Source: Microvias
Chapter
1 Introduction to Microvia and WLCSP Technologies
1.1 Semiconductor Industry Update The se...
118 downloads
1777 Views
12MB Size
Report
This content was uploaded by our users and we assume good faith they have the permission to share this book. If you own the copyright to this book and it is wrongfully on our website, we offer a simple DMCA procedure to remove your content from our site. Start by pressing the button below!
Report copyright / DMCA form
Source: Microvias
Chapter
1 Introduction to Microvia and WLCSP Technologies
1.1 Semiconductor Industry Update The semiconductor industry is firing on all cylinders. Worldwide semiconductor sales are predicted to grow by a combined annual growth rate (CAGR) of 16.2 percent from 2000 to 2004, reaching $316.2 billion as shown in Fig. 1.1. Sales remain strong across all product segments, including digital signal processors (DSPs), standard-cell applicationspecific integrated circuits (ASICs), dynamic random access memories (DRAMs), microprocessors, and flash and telecom analog chips. The applications driving booming chip demand are personal computers, networking equipment, and wireless communications. The networking hardware market will grow to $104 billion by 2004, while the worldwide number of broadband subscribers will climb to $61 billion during the same time frame. The wireless communications market will reach $132 billion by 2004, while the total number of cellular handsets (cell phones) shipped will soar to 1.4 billion units. The region of fastest growing equipment consumption is the Asia Pacific region, led by Taiwan and South Korea, which have consumed $6.8 billion and $3.4 billion worth of equipment, respectively, in 2000. The Asia Pacific region will surpass the Americas as the largest equipment consumer by 2001, while Europe and Japan will both approach the $10 billion mark by 2002. There are almost forty 12-in. semiconductor fabrications (FABs) in the world. Two-thirds of these FABs are located in the Asia Pacific region, led by Taiwan, Japan, and South Korea.
1
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
2
Chapter One
Figure 1.1
Worldwide semiconductor revenue growth.
1.2 System-on-a-Chip (SOC) One of the 12-in. FABs’ future semiconductor integrated circuit (IC) products is system-on-a-chip (SOC), which contains diverse functions on a single, large, and complex chip. These chip designs and build cycles usually are long and require multiple design passes to complete. The advantages of SOC are performance, small system form factor, and potentially low system cost. The challenges of SOC are: (1) to deal with the cost of large ICs, the slowdown in the reduction of cost per transistor as a result of very low IC yields, and the very high wafer FAB costs that are estimated to be in the range of $3 to 5 billion; (2) to integrate the intellectual property from multiple, possibly independent sources, with attendant interoperability, integration, and liability hurdles; and (3) to meet the mixed-signal requirements of future products, mixed technology systems, design issues, and limitation of on-chip performance that the industry faces for the first time. 1.3 System-on-a-Package (SOP) Based on the trends in the semiconductor industry, IC packaging1–12 can look forward to solid growth in the next few years, as shown in Table 1.1. It can be seen that chip scale packages (CSPs) have the largest percentage of CAGR, followed by the ball grid array (BGA) and the direct chip attach (DCA). Although there is no way to determine the exact
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
TABLE 1.1
3
IC Package Forecast by Package Family
Package units (M)
1999
2000
2001
2002
DIP
9,413
8,880
8,838
7,974
2003 8,126
2004 8,165
−2.80%
CAGR
SO
40,163
43,803
49,167
52,123
58,793
63,477
9.59%
CC
3,430
3,570
3,851
3,890
4,092
4,276
4.51%
QFP
6,371
7,241
8,138
8,939
9,794
10,912
11.36%
PGA
244
268
294
333
397
428
11.90%
BGA
1,742
2,491
3,311
4,244
5,237
6,205
28.92%
CSP
1,180
2,402
3,762
5,395
7,516
9,908
53.04%
DCA
5,588
6,257
7,099
7,999
9,201
10,311
13.04%
Total
68,130
74,914
84,461
90,898
103,157
113,683
10.78%
total revenue of IC packaging, 10 percent of the total semiconductor revenue is a reasonable guess for the total IC packaging revenue. In that case, the total revenue of IC packaging should be $32 billion by 2004. For very high-volume and simple applications, SOC is particularly appropriate. However, for mixed technologies, lower volumes, and the integration of passives, SOP is the most appropriate. SOP is an attractive alternative to SOC design complexity and uses a lower-risk approach that permits the use of mature semiconductor and packaging technologies and standard chip-to-package attach methods. In the case of printed circuit board (PCB) design of multiple packaging technologies such as wire bonding, DCA, CSP, and BGA, it is often clear that designing and manufacturing a PCB containing all these diverse technologies can be expensive and time consuming. Moreover, in these designs, clusters of functionally related components can be identified as ideal candidates for functional subassemblies—a microprocessor and its buffer memory, an input/output (I/O) processor and interface chips. Packaging technology has now progressed to the point where these “systems” (subsystems) can be contained on an independent package called a few-chip module (FCM). This package can be assembled and tested separately, often resulting in saving of PCB space and cost, simplication of the substrate carrier (either organic or ceramic), and lower overall packaging costs. Electrical performance is enhanced through shorter interconnections of chip on SOP. The use of reference planes allows isolation of critical nets. Impedance/coupling levels can be controlled. Current design ground rules allow regions of very dense wiring to permit interconnection of high chip pin counts. Using glass-ceramic or organic materials offers the fastest propagation speeds and lowest line resis-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
4
Chapter One
tances. The close physical proximity of the components mounted on SOP can minimize operating temperature deltas and permit thermal tracking, improving system performance. Use of an FCM allows designers to optimize that set of components for performance through functional subsystem testing prior to PCB assembly, allowing simplification of board test. The compacting of several electrical functions into SOP usually leads to some thermal challenges. Unless power and airflow levels are such that no heat management is necessary, the package components will have their own unique solutions. On simple two (or three)-chip SOPs, separate heat spreaders can be attached to each chip, depending on its power level. If space permits, an advanced thermal compound can be dispensed onto each component and a full module cap can be used. The differing expansion rates of each element in the SOP demand mechanical isolation for thermal management. Often, common heat sinking approaches can be used with SOP to minimize the number and handing of individual thermal solutions. Both direct lid attachment (DLA) and thermal paste solutions can be used when components are closely spaced; individual applications will require differing solutions. 1.4 Microvia and Wafer-Level Chip-Scale Package (WLCSP) As mentioned earlier, CSP will have the largest percentage of CAGR in the future of IC packaging. WLCSP is not only one of the CSPs, but the real CSP. Also, WLCSP is considered potentially the most cost-effective and reliable package. There are more than 30 different types of WLCSP reported in the literature, and their advantages and disadvantages have already been discussed.1–4 Just like many other new technologies, however, WLCSP still faces many critical issues (only solder-bumped WLCSP will be considered13–30): ■
The infrastructure of WLCSP is not well established.
■
The standard of WLCSP is not well established.
■
WLCSP expertise is not commonly available.
■
Bare wafer is not commonly available.
■
Bare wafer handling is delicate.
■
The Cost for poor-yield IC wafers is high.
■
Wafer bumping is still too costly.
■
There is a high cost for low wafer-bumping yield, especially for highcost dies.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
5
■
Wafer-level redistribution is still too costly.
■
There is a high cost for low wafer-level redistribution yield, especially for high-cost dies.
■
Troubles can occur with system makers if the die shrinks.
■
Test at speed and burn-in at high temperature on a wafer are difficult.
■
Single-point touch-up on the wafer is difficult.
■
PCB assembly of WLCSP is difficult.
■
Solder joint reliability is critical.
■
Microvia build-up PCB affects WLCSP solder joint reliability.
■
Alpha particle emission occurs through the lead-bearing solder on WLCSP.
■
Lead-free solder regulations have an impact on WLCSP.
■
Who should do the WLCSP? IC foundries or bump houses?
■
What are the cost-effective and reliable WLCSPs and for what IC devices?
■
How large is the WLCSP market?
■
What is the life cycle of WLCSP?
One of the unique features of most WLCSPs is the use of a metal layer to redistribute the very fine-pitch peripheral-arrayed pads on the chip to much larger-pitch area-arrayed pads with much taller solder joints on the PCB or substrate, as shown in Figs. 1.2 through 1.5. Figure 1.2 shows the wafer-level redistribution. Figure 1.3 shows a cross section of the redistribution. Figure 1.4 shows a typical cross section of the WLCSP assembled on a PCB, and Fig. 1.5 shows the cross section of the WLCSP-PCB assembly in more detail. In this book a few new solder-bumped flip-chip WLCSPs will be discussed in Chap. 10. Also, solder developments for the next-generation high-density interconnects will be presented in Chap. 9. In general, with WLCSPs, the underfill encapsulant may not be necessary (as shown in Fig. 1.4) and the demands on the PCB or substrate are relaxed. Since there is no underfill for most of the WLCSP assemblies, solder joint reliability becomes one of the most critical issues. Chapter 12 will address the solder joint reliability issues. A few new and high-throughput processes for assembling WLCSPs on PCB or substrate will be discussed in Chap. 11. For solder-bumped flip chip on low-cost substrate or PCB applications, even with wafer-level pad redistribution (from peripheral array to area array) to relax the pressure on PCB or substrate, in many cases
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
6
Chapter One
Figure 1.2
Wafer-level redistribution on a peripheral-arrayed
chip.
one to two or even three to four build-up layers with microvias are needed to fan out the circuitry. Chapters 3 through 7 will present, respectively, five different methods of forming the microvias, namely mechanical numerical control (NC) drilling, laser drilling, photo defining, etching, and conductive-material fill. A few very special and novel microvia build-up substrates for solder-bumped flip chip in packages are discussed in Chap. 8. Some necessary fundamental knowledge for making the conventional PCB or substrate is presented in Chap. 2. In this chapter, microvia build-up PCBs or substrates will be briefly discussed. However, since packaging cost is the most important issue, the WLCSP costs will be discussed first.
A typical cross section of the wafer-level redistributed chip.
Figure 1.3
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
Figure 1.4
7
PCB assembly of the WLCSP.
1.5 WLCSP Costs Since 100 percent perfect wafers cannot be made at high volume today, the true IC chip yield YT plays the most important role in cost analysis. Also, the physical possible number of undamaged chips Nc stepped from a wafer is needed for cost analysis, since (YTNc) is the number of truly good dies on a wafer. Nc is given by1, 2, 16
Figure 1.5
PCB assembly of the WLCSP (enlarged view).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
8
Chapter One
[φ − (1 + θ)兹A/θ 苶]2 Nc = π ᎏᎏᎏ 4A
(1.1)
A = xy
(1.2)
x θ=ᎏ ≥1 y
(1.3)
where
and
In Eq. (1.1) through (1.3), x and y are the dimensions of a rectangular chip (in mm), with x no less than y; θ is the ratio between x and y; φ is the wafer diameter (mm); and A is the area of the chip (in mm2). For example, for a 200-mm wafer with A = 10 × 10 = 100 mm2, then Nc ∼ 255 chips. 1.5.1 Wafer redistribution costs
Wafer-level redistribution is the heart of the WLCSPs, since only a handful of companies have the area-arrayed IC technology. The cost of wafer-level redistribution is affected by the true yield YT of the IC chip, the wafer-level redistribution yield YR , and the good die cost CD. The actual wafer-level redistribution cost per wafer CR is CR = CWR + (1 − YR)YTNcCD
(1.4)
where CWR is the wafer-level redistribution cost per wafer (ranging from $50 to $200), YR is the wafer-level redistribution yield per wafer, CD is the good die cost, Nc is given in Eq. (1.1), and YT is the true IC chip yield after at-speed/burn-in system tests. Again, it can be seen that the actual wafer-level redistribution cost per wafer depends not only on the wafer-level redistribution cost per wafer but also on the true IC chip yield per wafer, wafer-level redistribution yield per wafer, and good die cost. Wafer-level redistribution yield YR plays a very important role in WLCSP. The wafer-level redistribution yield loss (1 − YR) could be due to: 1. More process steps 2. Wafer breakage 3. Wafer warping
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
9
4. Process defects such as spots of contamination or irregularities on the wafer surface 5. Mask defects such as spots, holes, inclusions, protrusions, breaks, and bridges 6. Feature size distortions 7. Pattern misregistration 8. Lack of resist adhesion 9. Overetching 10. Undercutting 11. Incomplete etching 12. Wrong materials It should be noted that rework of wafer-level redistribution is very difficult if not impossible. It has to be right the first time; otherwise, someone has to pay for it! The uses of Eq. (1.1) and (1.4) are shown in the following examples. If the die size of a 200-mm wafer is 100 mm2, true IC chip yield per wafer is 80 percent (since the importance of YT has been shown in Refs. 1, 2, and 28, only one value of YT will be considered in this study), wafer-level redistribution yield per wafer is 90 percent, wafer-level redistribution cost per wafer is $100, and die cost is $100 (e.g., microprocessors), then from Eq. (1.1), Nc = 255, and from Eq. (1.4), the actual wafer-level redistribution cost per wafer is $2140. For the same size of wafer, if the die cost is $5 (e.g., memory devices), then the actual waferlevel redistribution cost per wafer is $202. It is noted that for both cases the actual wafer-level redistribution cost per wafer is much higher than the wafer-level redistribution cost (CWR = $100)! On the other hand, if the wafer-level redistribution yield is increased from 90 percent to 99 percent, then the actual cost for redistributing the microprocessor wafer is reduced from $2140 to $304 and for redistributing the memory wafer it is reduced from $202 to $110.2 (Table 1.2). Thus, wafer-level redistribution yield plays an important role in the cost of wafer-level redistribution and the wafer-level redistribution houses should strive to make YR > 99 percent, especially for expensive good dies. 1.5.2 Wafer bumping costs
Wafer bumping is the heart of solder-bumped WLCSPs. The cost of wafer bumping is affected by YT, CD, YR and the wafer-bumping yield YB. The actual wafer-bumping cost per wafer CB is CB = CWB + (1 − YB)YRYTNcCD
(1.5)
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
99%
90%
90%
90%
$1956
$4096
$3876
$20.08
Wafer-level bumping yield
Actual wafer-level bumping cost
Total actual cost of WLCSP per wafer
Hidden cost of WLCSP per wafer
Actual cost of WLCSP per good die
$11.98
$2223.60
$2443.60
$303.60
90%
90%
$11.98
$2223.60
$2443.60
$2139.60
$304
$3.07
$405.96
$625.96
$321.96
$2.03
$193.80
$413.80
$211.80
$202
$1.62
$111.18
$1.62
$111.18
$331.18
90% $220.98
99%
$331.18
99%
99%
$1.18
$20.30
$240.30
$130.10
$110.20
$129.18
Number of physically possible dies on wafer
$2140
255
255
Wafer-level bumping cost
Actual wafer-level redistribution cost
$120
$120
Wafer-level redistribution cost
Wafer-level redistribution yield
80% $100
80% $100
IC chip yield
99%
$5
$100
Good die cost
99%
Memory device
Item
WLCSP Cost Analysis Microprocessor device
TABLE 1.2
Introduction to Microvia and WLCSP Technologies
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
10
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
11
where CWB is the wafer-bumping cost per wafer (ranging from $25 to $250), YB is the wafer-bumping yield per wafer, YR is the wafer-level redistribution yield per wafer, CD is the good die cost, Nc is given in Eq. (1.1), and YT is the true IC chip yield after at-speed/burn-in system tests. Again, it can be seen that the actual wafer-bumping cost per wafer depends not only on the wafer-bumping cost per wafer but also on the true IC chip yield per wafer, wafer-bumping yield per wafer, good die cost, and wafer-level redistribution yield per wafer. Just like YR, wafer-bumping yield YB plays a very important role in WLCSP. The wafer-bumping yield loss (1 − YB) could be due to: 1. Wrong process 2. Different materials 3. Too tall or short of a bump height 4. Not enough shear strength 5. Uneven shear strength 6. Broken wafers or dies 7. Solder bridging 8. Damaged bumps 9. Missing bumps 10. Scratching of the wafer For the previous example, if the wafer-bumping yield per wafer is 90 percent and wafer-bumping cost per wafer is $120, then the actual wafer-bumping costs per (microprocessor) wafer are, respectively, $1956 if YR = 90 percent and $2139.60 if YR = 99 percent, and the actual wafer bumping costs per (the memory) wafer are, respectively, $211.80 if YR = 90 percent and $220.98 if YR = 99 percent (Table 1.2). Again, it should be noted that the actual wafer-bumping cost per wafer is much higher than the wafer-bumping cost (CWB = $120). On the other hand, if the wafer-bumping yield is increased from 90 percent to 99 percent, then the actual costs for bumping the microprocessors wafer are, respectively, $303.60 if YR = 90 percent and $321.96 if YR = 99 percent, and the actual costs for bumping the memory wafer are, respectively, $129.18 if YR = 90 percent and $130.10 if YR = 99 percent. Thus, wafer-bumping yield plays an important role in the cost of wafer bumping and the wafer-bumping houses should stride to make YBYR > 99 percent, especially for expensive good dies. If there is no wafer-level redistribution, then there is no wafer redistribution yield loss, i.e., YR = 1, and Eq. (1.5) degenerates to that shown in Refs. 1 and 2.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
12
Chapter One
1.5.3 Wafer redistribution and wafer-bumping costs
Based on the foregoing discussions, the total actual cost for solderbumping and wafer-level redistribution CBR becomes CBR = CWBR + (1 − YRYB)YTNcCD
(1.6)
CWBR = CWR + CWB
(1.7)
where
is the sum of wafer-level redistribution cost and wafer-bumping cost CWBR usually charged by the wafer-bumping houses. For our example, the total actual costs of the microprocessor WLCSP are: CBR = $4096 if YR = YB = 90 percent; CBR = $2443.60 if YR = 90 percent and YB = 99 percent or YR = 99 percent and YB = 90 percent; and CBR = $625.96 if YR = YB = 99 percent. The total actual costs of the memory WLCSP are: CBR = $413.80 if YR = YB = 90 percent; CBR = $331.18 if YR = 90 percent and YB = 99 percent or YR = 99 percent and YB = 90 percent; and CBR = $240.30 if YR = YB = 99 percent (Table 1.2). Thus (1) for both devices, the actual WLCSP costs are higher than the cost ($100 + $120 = $220) charged by the redistribution-bumping houses; (2) this is even more so for the more expensive dies; and (3) YR and YB play very important roles in WLCSP and YRYB > 99 percent is a must for WLCSP to be competitive. 1.5.4 WLCSP hidden costs
The hidden cost per wafer is defined as the difference between the actual wafer-bumping and wafer-level redistribution cost, and the waferbumping and wafer-level redistribution cost charged by the waferbumping houses. From Eq. (1.6), the hidden cost per wafer for solder-bumped WLCSP CH is given as CH = CBR − CWBR
(1.8)
CH = (1 − YRYB)YTNcCD
(1.9)
or
It can be seen that, if YR = YB = 1, then there is no hidden cost (CH = 0) in solder-bumped WLCSP, meaning the wafer-bumping houses are perfect in doing the wafer-level redistribution and wafer bumping. Unfortunately, they cannot and never will be perfect, which is what makes the costs of wafer-level redistribution and wafer bumping so expensive, especially for expensive good dies.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
13
For our example, the hidden costs of the microprocessor WLCSP are: CH = $3876 if YR = YB = 90 percent; CH = $2223.60 if YR = 90 percent and YB = 99 percent or YR = 99 percent and YB = 90 percent; and CH = $405.96 if YR = YB = 99 percent. The hidden costs of the memory WLCSP are: CH = $193.80 if YR = YB = 90 percent; CH = $111.18 if YR = 90 percent and YB = 99 percent or YR = 99 percent and YB = 90 percent; and CH = $20.30 if YR = YB = 99 percent (Table 1.2). The fact that someone has to pay for (or share) the hidden costs is one of the major reasons why solder-bumped WLCSP is not very popular today. 1.5.5 WLCSP cost per good die
The actual wafer-bumping and wafer-level redistribution cost per good die CBR/D can be determined by CBR/D = CBR/YTNc
(1.10)
CBR/D = CWBR/YTNc + (1 − YBYR)CD
(1.11)
or
For our example, the actual WLCSP costs per the good microprocessor die are: CBR/D = $20.08 if YR = YB = 90 percent; CBR/D = $11.98 if YR = 90 percent and YB = 99 percent or YR = 99 percent and YB = 90 percent; and CBR/D = $3.07 if YR = YB = 99 percent. The total actual WLCSP costs per the good memory die are: CBR/D = $2.03 if YR = YB = 90 percent; CBR/D = $1.62 if YR = 90 percent and YB = 99 percent or YR = 99 percent and YB = 90 percent; and CBR/D = $1.18 if YR = YB = 99 percent (Table 1.2). Comparing with the wire bonding technology, these costs are much too high for solder-bumped WLCSP to be competitive, unless it is compensated for by performance, density, and form factor. Thus, again, YRYB >> 99 percent is a must for WLCSP to be popular. 1.5.6 Wafer-level underfill costs
For some special applications, such as portable electronic products under drop (shock) and vibration kinds of operation conditions, underfills are needed for ensuring the solder joint reliability of WLCSPs. Recently, in order to increase throughput and reduce production time, the research in wafer-level underfill materials and process has been very active.20 For WLCSP, in this process, the underfill is deposited on the entire solder-bumped wafer prior to dicing. During surface-mount technology (SMT) assemblies, the singulated chip is processed as in standard flip chip reflow operations. The key difference is that the pre-underfilled (with build-in flux) solder-bumped chip will be reflowed and cured concurrently between the chip and the organic substrate.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
14
Chapter One
The actual wafer-level underfill cost per wafer CU can be determined by CU = CWU + (1 − YU)YBYRYTNcCD
(1.12)
where CWU is the wafer-level underfill cost per wafer and YU is the wafer-level underfill yield per wafer. The wafer-level underfill yield loss (1 − YU) could be due to: 1. More wafer process steps 2. Wrong process 3. Wrong materials 4. Dicing 5. Nonuniformity 6. Incompletely cured underfill 7. Damage to solder bumps 8. Breaking of the wafer 9. Scratching of the wafer 10. Too high a thermal expansion coefficient 11. Too low a modulus The actual wafer-level underfill cost per good die CU/D can be determined by CU/D = CWU/YTNc + (1 − YU)YBYRCD
(1.13)
Thus, from the cost point of view, wafer-level underfill is not a good idea and makes solder-bumped WLCSP even more expensive. It can be seen from the first term of the right side of Eq. (1.13) that the underfill costs of the good dies are increased because some of the expensive underfills are wasted on the bad dies. Also, the hidden cost of wafer-level underfill per good die is high and is shown in the second term of Eq. (1.13). It should be pointed out that, in most of the conventional solderbumped flip chip on low-cost substrate applications, the underfill operation is usually applied to the individual dies after the system test of the assemblies.1–5 The reasons are: (1) it is easy to rework; (2) underfill is needed for only the good dies; and (3) there is no chance to damage the very expensive wafer. Also, from the process point of view, waferlevel underfill will reduce the self-alignment characteristic (which is so unique) of solder-bumped flip chip technology.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
15
If there is no wafer-level pad redistribution operation, then the actual wafer-level underfill cost per wafer can be determined by CU = CWU + (1 − YU)YBYTNcCD
(1.14)
Also, the actual wafer-level underfill cost per good die CU/D without wafer-level pad redistribution can be determined by CU/D = CWU/YTNc + (1 − YU)YBCD
(1.15)
Again, from both cost and process points of view, wafer-level underfill is not a good idea for solder-bumped flip chip on low-cost substrates. 1.5.7 Summary
More than 20 different critical issues regarding WLCSP have been mentioned. The most important issue of WLCSP (cost) has been analyzed in terms of the true IC chip yield, wafer-level redistribution yield, wafer-bumping yield, wafer-level underfill yield, and die size and cost. Also, useful equations in terms of these parameters have been presented and demonstrated through examples. Some important results are summarized as follows. ■
IC chip yield YT plays the most important role in WLCSP. If YT is low for a particular IC device, then it is not cost effective to house the IC with WLCSP, unless it is compensated for by performance, density, and form factor.
■
Wafer-level redistribution yield YR plays the second most important role in WLCSP. Since this is the first postwafer processing after the IC FAB, the wafer-level redistribution houses should strive to make YR > 99 percent (99.9 percent is preferred). Otherwise, the subsequent steps will be made very expensive by wasting of the material and process on the damaged dies.
■
Wafer-bumping yield YB plays the third most important role in WLCSP. The wafer-bumping house should strive to make YRYB > 99 percent (99.9 percent is preferred) to minimize the hidden cost, since they cannot afford to damage the already redistributed good dies.
■
Based on cost and process points of view, wafer-level underfill is not a good idea for solder-bumped flip chip on low-cost substrates.
1.6 Microvia Microvias are the keys to making low-cost and high-density PCBs and substrates. In order to make cost-effective PCB and substrates, the
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
16
Chapter One
sequential buildup (SBU) fabrication technique is a must. This is done by adding a minimum of one layer of dielectric to the double-sided or multilayer core. Non-through-hole microvias are selectively formed to reclaim real estate and are used to accommodate the fine I/O pitch and redistribute circuits from the chip to the internal layers of the PCB, reduce PCB layer count and size, and enhance electrical performance. By IPC’s definition, holes of 6 mils (0.15 mm) or less on PCBs and substrates are called microvias. There are many advantages of microvia:31–78 (1) it requires a much smaller pad, which saves the board size and weight; (2) more chips can be placed in less space or a smaller PCB, which results in a low cost; and (3) electrical performance improves as well, since the parasitic capacitance is increased due to the smaller via length and diameter and the inductance is reduced due to the shorter pathway created by the microvia compared to the plated through-hole (PTH).31–37 According to a recent study by TechSearch International, the market for microvia substrates will reach $1.6 billion this year. That number is expected to grow to $8.6 billion by 2005. Currently, 75 companies around the world are producing microvia substrates. Japan is the world leader, with more than 50 percent of the world’s microvia production. Europe and the Asia Pacific region come in second in microvia production. Most of the products that use microvia technology are mobile phones (Fig. 1.6), notebook computers, and other handheld products. The U.S. will not have high volume production until after 2000. The reason is that most U.S. companies are currently focusing on high-value applications like workstations, servers, and network systems. Table 1.3 shows the usage of microvias in different business sectors. It can be seen that the largest market is in personal communications such as the mobile phone (Fig. 1.6). Figures 1.7 through 1.10 show a few examples (by Intel and Mitsubishi) of using the microvia build-up substrates for solder-bumped flip chips, usually microprocessors and ASIC applications. Figure 1.11 shows a microvia build-up PCB with two thinfilm metal layers by X-LAM, which will be discussed in Chap. 8. 1.6.1 Categories of vias
Typical via hole diameters range from 50 to 300 µm and are divided into three categories. Blind vias. Blind vias are located on the outer layer of the top and bottom of the circuit board and are formed to a depth at which they make contact with the first inner layer. The depth of this hole usually does not exceed 1 aspect ratio (hole diameter).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
17
Figure 1.6 Mobile phone with microvia build-up PCB. (Courtesy of Samsung)
Buried vias. Buried vias are holes that are plated within the core of the circuit board without access to the surface on either side of the board. These holes are formed before the board is laminated. The innerlayer material has the holes created by a through-hole processing method. The inner layers may be stacked several layers high during this hole formation process. Through-hole vias. Through-hole vias are formed through the entire thickness of the board. These vias are used as interconnect or as mounting locations for components. Basically, there are five major processes for microvia formation: (1) NC drilling; (2) laser via fabrication including CO2 laser, yttrium aluminum garnet (YAG) laser, and Excimer laser, (3) photo-defined vias, wet or dry; (4) etch via fabrications, including chemical (wet) etching and plasma (dry) etching; and (5) conductive-ink-filled vias, wet or dry. In general, even though photo-defining and chemical and plasma etching processes can make microvias in very high throughput, laser drills can make finer vias. 1.6.2 Microvias made by mechanical NC drilling
Currently, NC drilling is the most common process for generating holes on the PCB. However, NC drilling is technically limited to hole sizes of
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Cisco, Lucent, Alcatel, Nortel, Sun, Ericsson, NEC, Schlumberger, Agilent, HP
Mainly North American and some European, with limited opportunity in Asia Pacific
Accelerating growth in largearea boards as multiple highleadcount ASICs drop to 1-mm pitch and below.
Players
Geography
Direction
Very rapid growth driven by both demand and conversion to CSP/microvia by majors. Cellphones will become smaller due to baseband and RF integration and despite multimode function.
Mainly Japan and Southeast Asia; now rapidly becoming global with Europe and U.S.
Samsung and all Japanese cellphone makers (Panasonic, NEC, Sharp, Fujitsu, Kyocera, etc.); Motorola, Nokia, and Ericsson (combined 67% of market and rapidly converting to microvia— 104 million units 1997)
$180 million → $970 million
$18 million → $450 million
Market size
Personal communications Cellphones, pagers, personal communications, handheld global positioning systems (GPSs), satellite phones
Workstations, servers, processor modules, transmission, switching, router boards, test equipment
Computing and data communications
Usage of Microvias in Different Business Sectors
Products
TABLE 1.3
Digital imaging
Steady growth in camcorders and cost reduction through integration. Digital cameras going from 2 million units to 8 million units per year in 2002, and converting from ceramic to microvia.
Mainly Japan, with Japan remaining dominant
JVC Victor, Sony, Panasonic, Kodak (9 million camcorders and 2 million digital cameras in 1997)
$125 million → $280 million
Camcorders, digital cameras, digital receivers
Introduction to Microvia and WLCSP Technologies
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
18
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
19
Figure 1.7 Intel’s microprocessor supported by a microvia build-up substrate.
Figure 1.8
Schematic of Intel’s microvia build-up substrate.
Figure 1.9
Mitsubishi’s microvia build-up substrate.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
20
Chapter One
Mitsubishi’s solder-bumped flip chip plastic ball grid array (PBGA) package with microvias.
Figure 1.10
Figure 1.11
Schematic of X-LAM’s thin-film metal layer substrate.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
21
200 µm and up (not microvias). Although smaller holes may be possible, these would come at the cost of significant productivity (such as minimal stack height). In addition, the blind vias are virtually impossible where typical dielectric thickness is 50 µm or less.38 In general, mechanical drilling cannot make microvias. However, it should be pointed out that some special machines are being designed to drill very small vias. For example, Excellon Automation have been developing drilling machines that can drill vias as small as 4 mils (100 µm) in diameter. For more information on mechanical NC drilling, please read Chap. 3. 1.6.3 Microvias made by laser drilling
Laser drilling can be a single or multiple via generation process that replaces the existing mechanical drilling process. Laser drilling differs from mechanical drilling in that the focused beam used to create the holes can produce smaller holes than those produced by conventional drilling. One of the most important advantages of laser drilling is that it is compatible with many copper-clad or unclad dielectrics and reinforced or nonreinforced PCBs. Laser drilling can be used to create both blind vias and holes. The process follows standard multilayer and is capable of resolving smaller features. Low productivity is one of the weaknesses of laser drilling; that is, one beam produces one blind via at a time.31 Laserdrilled microvias have been reported by several authors,39–51 and a typical PCB including a blind via is shown in Fig. 1.12. Several laser processes have been developed to generate small via holes; these are categorized as Excimer laser, YAG laser, and CO2 laser. The CO2 lasers have significantly higher productivity for holes larger than 70 µm in diameter. They can ablate more than 15,000 (100 µm diameter) holes through 50-µm-thick dielectric in 1 min. In general,
Figure 1.12
laser.
Via (75 µm) on 45-µm resin by UV:YAG
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
22
Chapter One
carbon dioxide laser is used to drill holes on the dielectric layer and not to drill holes on copper, because the visible wavelength (1060 nm) of CO2 is too large to have enough energy to penetrate the copper at high speed. Today, the companies that supply the CO2 laser drilling machines are Hitachi, Lumonics, Panasonic (Matsushita), Mitsubishi, and Sumitomo. On the other hand, the ultraviolet (UV):YAG laser, with smaller wavelengths (365 to 255 nm) and much higher energy, is used to drill holes on the copper and dielectric (the so-called imaging method) at a much lower speed. UV:YAG lasers have demonstrated great productivity through both dielectric and copper layers, but for both processes ablation time is proportional to hole diameter and neither process is therefore competitive above 100 µm diameter. Today, ESI, Excellon, Exotech, Hitachi, and Sumitomo supply the UV/Nd:YAG laser machines. Also, Hitachi and Lumonics of Canada now offer a combination of Nd:YAG/CO2 laser machines. The excimer laser has a wavelength of 248 nm with krypton fluoride (KrF) and of 193 nm with argon fluoride (ArF). Excimer lasers can generate holes smaller than 50 µm in diameter through dielectric or copper layers. Controlled-depth drilling is also possible, thus allowing blind vias to be created. The slow etch rate, however, makes this process impractical for microvia formation. Today, Litel, JPSA, and Tamarack supply UV:excimer machines, to which JPSA can add either T-CO2 or diamond CO2 laser heads. For more information about laser-drilled microvias, please read Chap. 4. 1.6.4 Photo-defined vias
In 1990, IBM at Yasu, Japan, commercially produced microvias using a modified liquid photoimageable dielectric (PID). Modern PID is either a liquid or dry film. For photovias with liquid photodielectric, the dielectric is curtain-coated and cured, microvias are exposed, and the dielectric is developed. Panel plating follows with patterning to create signal traces. For photovias with dry-film photodielectric, the dielectric is laminated, microvias are exposed, and the dielectric is developed. Panel plating follows with patterning to create signal traces.55 The equipment needed for photo-defined via technology includes exposure unit, developer, and wet process. The suppliers of exposure unit are Bacher, Byers, Colight, Csun, Dupont, Dynachem, Gyrex, HiTech, Mirmir, Morton, Olec, Optical Radiation, ORC, Peak Measuring, Tamarac, and Theimer. The suppliers of developer are Advanced Chemill Systems, ASI, Chemcut, Ciba-Geigy, Circuit Services, Danippon Screen, Glenbrook, James River, Lantronic, Microplate, Quan-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
23
tum, Rexham Graphics, and Technifax. The suppliers of wet process (develop-etch-strip) are ASI, Chemcut, Hollmuller, Lantronic, and Schmid. For more information about photo-defined microvias, please read Chap. 5. 1.6.5 Chemical (wet)- and plasma (dry)-etched vias
Microvias can be formed by various etching techniques. The most common etching technique is to use a microwave-gas plasma, which is a dry etching process. Wet etching by hot KOH has been used for polyimide films. Both methods are isotropic such that they etch inward while they etch down. On the positive side, these formation techniques involve mass via generation in that they form all vias at the same time without regard to number or diameter. Plasma etching and chemical etching can be extremely cost effective for generating high volumes of small holes in dielectric layers. The principle in this case is to create a mask, which defines the position and size of the holes. This may be achieved by using dry film to image and then etch a hole pattern in a copper layer, or simply by using the dry film as the etch mask by imaging and developing. In either case the process cost is derived by the number of holes in a given working area. All the holes are generated simultaneously, and the process time is dependent on how long it takes to erode or dissolve the unmasked dielectric. Plasma etching has the added benefit of removing organic contaminants, and with careful conditioning, the amount of slope (undercut) created in the hole can be minimized. Chemical etching is the lowest-cost process for generating small holes on dielectrics. Both plasma and chemical etching processes can create blind vias, usually using the target pad as a means of defining the bottom of the blind via.57–58 The dry etching process needs extra processes like plasma etching and copper thinning (etch-back) processes. Micro Via Hole (MVH) formation by gas-microwave plasma (GMP) has been promoted by Dyconex of Switzerland. Dyconex has sixteen licensees worldwide because it sells a basic plasma drill for $55,000, compared to a laser drill that costs from $500,000 and up or to a photoimaging facility that requires around $300,000. The plasma equipment can be found from Advanced Plasma Systems, Inc. or Plasma Etch Inc. For more information about etched microvias, please read Chap. 6. 1.6.6 Conductive-ink-filled vias
Conductive ink describes a single-layer dielectric with microvias formed by laser, photoimaging, or insulation displacement. A conduc-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
24
Chapter One
tive paste (or film) is used to fill the microvias and act as the conductive path between layers. Surface metallization may be accomplished either by laminating copper foil onto the dielectric surface or by chemical deposition. For more information about conductive-ink-filled microvias, please read Chap. 7. 1.6.7 Microvia production in Japan
Since more than half of the world’s microvia PCBs and substrates are made in Japan, it is interesting to note the status of some key manufacturers in this area. These are reported as follows. (See Table 1.4 for additional details.) Fujitsu Limited. Fujitsu’s FLD (Fujitsu Laminate and Deposit) buildup process is currently in production and utilizing photoimaging system. FLLD (Fujitsu Laminate with Laser via and Deposit) process is under development and utilizes a laser drilling system. The technology is capable of producing 50-µm copper lines with 50-µm spaces and 100-µm-diameter vias for packaging substrates. Fujitsu is changing from photovia to laser via for its next generation packaging substrates. Highly Accelerated Stress Test (HAST) and reliability test results are presented in Ref. 64. Hitachi Chemical Co. Hitachi has developed two types of PCBs, namely, HITAVIA Type 1 and Type 3 using metal clad B-stage insulation resin film (MCF). Type 1 is used for motherboards and liquid crystal display drivers; Type 3 is used for semiconductor packages such as PBGA. The interstitial via holes (IVHs) are formed using mechanically predrilled metal-clad film. A CO2 laser is used to etch the microvias. The technology is capable of producing 100-µm copper lines with 100-µm spaces for Type 1 and 50-µm lines with 50-µm spaces for Type 3. The size of vias can be 250 µm on 500-µm pads for both types. All passed the qualification tests.65 Ibiden. Ibiden has developed a double-sided four-layer build-up board using fully additive copper plating and photosensitive epoxy. This technology is capable of producing 75-µm lines with 75-µm spaces for motherboards and 35-µm copper lines with 35-µm spaces for packages. Using the photovia process, it is possible to make 150-µm-diameter via on 250-µm lands for motherboards and 80-µm-diameter via holes on 125-µm lands for packages.66 IBM at Yasu. The IBM (at Yasu) Surface Laminar Circuit (SLC) also uses liquid-dispensed photoimaged epoxy in the build-up layers on FR-4 or bismaleimide triazine (BT) substrates. The photo-sensitive epoxy
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
TABLE 1.4
25
Microvia Build-up PCB and Substrate Suppliers
Company Amitec
Via formation method Thin film
Via/pad diameter (µm)
Line/space (µm)
Maximum number of multilayers
25/50
15/15
2–4
ASTI
Laser
25/125
35/35
16
Canon
Laser
150/300
75/75
3+core+3
Compaq
Laser
75/195
75/30
10
Daisho Denshi
Laser
100/300
75/75
8
D. T. Circuit
B2it
200/400
75/75
4+core+4
Fujitsu
Photovia Laser
80/130 50/100
40/40 35/35
6 3+core+3
Hitachi Cable
Laser
50/80
25/25
2
Hitachi Chemical
Laser
100/125
50/50
10
Ibiden (IBSS)
Photovia Laser
85/125 150/250
40/40 75/75
4-2-4 10
IBM (HPCC)
Laser
50/100
28/33
9
IBM (SLC)
Photovia
100/150
50/50
3+core+3
JCI
Laser
100/160
40/40
8
JVC
Laser
150/250
60/60
2+core+2
K&S (X-Lam)
Thin film
25/54
18/14
2-4
Kyocera/JME
Photovia
50/100
30/30
4-8-4
Matsushita
Laser
100/125
50/50
4+core+4
Mitsubishi
Laser
75/125
30/30
3+core+3
Multek
Photovia
75/150
75/75
8
NEC
Photovia
40/60
20/20
3+core+3
NTK
Photovia Laser
90/130 50/130
35/35 40/40
3+core+3 9
Samsung
Photovia with laser
150/200
50/50
3+core+3
Sheldahl
Laser
25/140
50/37.5
Shinko
Laser
50/110
45/45
3+core+3
2
SMI
Photovia
95/135
37/37
2+core+2
STP
Photovia
100/200
75/75
1+8+1
Toppan
Photovia Laser
80/130 100–125/300
40/40 75/75
3+core+3 —
W. L. Gore
Laser
50/87
25/25
9
The number before and after the core is the number of build-up layers.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
26
Chapter One
resin is exposed and developed to form the via hole. The via diameter can be 100 µm and the land diameter can also be 100 µm. The line width and space can be 38 µm. The flip chip attached on SLC board has passed reliability tests with 100°C delta temperature cycling and temperature/humidity/bias test.67–70 JVC. The Victor Company of Japan (JVC) has produced the Variously Interconnected Layers (VIL) type of build-up PCB by applying thermosetting material to insulation and by the laser processing of via holes through the mask imaging method. Lines and spaces of 100 µm have been produced. JVC has succeeded in making a skip via hole as small as 280 µm in diameter.71 Matsushita. Matsushita has developed a unique stacked type of substrate technology called ALIVH, which is discussed in Sec. 7.3.30–33 Laser ablation (currently CO2 laser) and Cu paste are used for buried holes. It is reported that Matsushita’s share of the Japanese cellular phone market has risen to 60 percent with the introduction of ALIVH substrates. The company’s conductor line and space resolution are 50 µm and 50 µm, respectively.72 Reliability data for ALIVH-CSP have been shown in Ref. 63. NEC. NEC Toyama has developed a high-density microvia (µV) PCB for advanced microelectronic packaging application. The more advanced technology can produce 50-µm copper lines with 50-µm spaces. The via diameter can be 50 µm and land diameter can be 150 µm. The via is formed by laser processing. Most of the samples pass reliability tests, although there are less than 3 percent fails on the interconnection reliability test, MIL-STD-107G (−65°C for 30 min to +125°C for 30 min) after 500 cycles.73 Toshiba. Toshiba has introduced a unique Buried Bump Interconnection Technology (B2it). Silver paste is used to form conductive bumps on copper foil. Conically shaped bumps can penetrate the insulator and form a conductive path through the prepreg. The conductive lines and spaces, currently 75 µm in width each, are being formed by subtractive processing using photoresist. The “via” (bump) diameter is 200 µm and the land diameter is 400 µm. These are now under mass production.74 Recently, Toshiba and Dai Nippon Printing Co., Ltd formed a new start-up company called D. T. Circuit Technology Co., Ltd for making the B2it PCB and substrate. A summary of the line width and space width capabilities of these eight Japanese microvia manufacturers is shown in Fig. 1.13. It can be seen that Ibiden can make the finest lines and spaces. Figure 1.14 is a
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
Figure 1.13
27
Line/space width technologies for some Japanese companies.
summary of the microvia and pad diameter capabilities of the eight Japanese microvia manufacturers. The smallest via and pad can be manufactured by NEC Toyama Corporation. It should be pointed out that five (Hitachi, Ibiden, JVC, Matsushita, and Toshiba) of the eight Japanese companies have developed their own new materials for the microvia process and formation. Four
Figure 1.14
Via/pad diameter technologies for some Japanese companies.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
28
Chapter One
(Hitachi, JVC, Matsushita, and NEC) use laser drilling. Two (Ibiden and IBM-Yasu) use photoimaging, and Fujitsu is changing from photoimaging to laser drilling. Toshiba (D. T. Circuit) has changed from the conventional (drilling and plating) process to a new process. 1.6.8 Summary
In general, laser drilling can create the smallest holes. Photo-defined via technology has highest productivity. Laser drilling technology gains 70 percent of the microvia market because of its straightforward nature and compatibility with all kinds of materials (including clad laminates, copper-coated foil, and dielectrics). The photoimaging method is the second most popular technology used in making microvias. Japan is the leader in making microvias, and the U.S. is very well back. However, some U.S. companies are catching up. For example, Johnson Matthey is the largest supplier of microvias in North America. It has 10 laser drills (4 YAG to ablate copper for RCC processing and 6 CO2 units to remove dielectric). Johnson Matthey’s electronic materials division was sold to Allied Signal Electronic Materials unit in August 1999. Allied Signal sold its laminate systems business to Rutgers AG, based in Essen, Germany, in order to enter higher-margin specialty segments. 1.7 A Note on High-Speed and High-Density Interconnects In Ref. 77, IPC-2141 gives the equations for estimating the characteristic impedance for some very simple circuits. Since these are approximate formulas, very often they lead to great errors, especially for high-speed and high-density interconnects. For example, for the simplest case (surface microstrip) shown in Fig. 1.15, with T = 35 µm, H = 794 µm, W = 3300 µm, εr = 4.2, IPC-2141’s equation underpredicts the characteristic impedance by almost 30 percent. In this book, some useful design charts for the surface microstrip, differential edge-coupled surface microstrip, embedded microstrip, differential microstrip, embedded stripline, differential symmetrical broadside-coupled stripline, differential symmetrical edge-couple centered-embedded stripline, and surface microstrips are shown in Figs. 1.15 through 1.26. It should be noted that all the data to make the curves are determined (with εr = 4.2) from numerical simulations of the Maxwell equations and checked randomly with some well-known solutions such as those given in Ref. 78. In these charts, Z0 is the characteristic impedance and Zdiff ⬵ 2 × Z0o, where Z0o is the odd-mode impedance.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
Figure 1.15
29
Characteristic impedance of a surface microstrip (εr = 4.2).
Figure 1.16 Differential impedance of a differential edge-coupled surface microstrip (εr = 4.2).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
30
Chapter One
Figure 1.17 Differential impedance of a differential edge-coupled surface microstrip (εr = 4.2).
Figure 1.18
Characteristic impedance of a embedded microstrip (εr = 4.2).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
31
Figure 1.19 Differential impedance of a differential centered-embedded microstrip (εr = 4.2).
Differential impedance of a differential centered edge-coupled embedded microstrip (εr = 4.2).
Figure 1.20
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
32
Chapter One
Figure 1.21
Characteristic impedance of an embedded stripline (εr = 4.2).
Figure 1.22 Differential impedance of a differential symmetrical broadsidecouple stripline (εr = 4.2).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
33
Figure 1.23 Differential impedance of a differential symmetrical embeddedcentered stripline (εr = 4.2).
Differential impedance of a differential symmetrical embeddedcentered stripline (εr = 4.2).
Figure 1.24
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
34
Chapter One
Figure 1.25
Capacitance of surface microstrips (εr = 4.2).
Figure 1.26
Inductance of surface microstrips (εr = 4.2).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
35
1.8 References 1. Lau, J. H., Low-Cost Flip Chip Technologies for DCA, WLCSP, and PBGA Assemblies, McGraw-Hill, New York, 2000. 2. Lau, J. H., and S.W.R. Lee, Chip Scale Package, Design, Materials, Process, Reliability, and Applications, McGraw-Hill, New York, 1999. 3. Lau, J. H., C. Wong, J. L. Prince, and W. Nakayama, Electronic Packaging, Design, Materials, Process, and Reliability, McGraw-Hill, New York, 1998. 4. Lau, J. H., and Y.-H. Pao, Solder Joint Reliability of BGA, CSP, Flip Chip, and Fine Pitch SMT Assemblies, McGraw-Hill, New York, 1997. 5. Lau, J. H., Flip Chip Technologies, McGraw-Hill, New York, 1996. 6. Lau, J. H., Ball Grid Array Technology, McGraw-Hill, New York, 1995. 7. Lau, J. H., Chip on Board Technologies for Multichip Modules, Van Nostrand Reinhold, New York, 1994. 8. Lau, J. H., Handbook of Fine Pitch Surface Mount Technology, Van Nostrand Reinhold, New York, 1994. 9. Frear, D., H. Morgan, S. Burchett, and J. Lau, The Mechanics of Solder Alloy, Van Nostrand Reinhold, New York, 1994. 10. Lau, J. H., Thermal Stress and Strain in Microelectronics Packaging, Van Nostrand Reinhold, New York, 1993. 11. Lau, J. H., Handbook of Tape Automated Bonding, Van Nostrand Reinhold, New York, 1992. 12. Lau, J. H., Solder Joint Reliability, Theory and Applications, Van Nostrand Reinhold, New York, 1991. 13. Garrou, P., “Wafer Level Chip Scale Packaging (WL-CSP): An Overview,” IEEE Trans. Adv. Packaging, 23(2): 198–205, May 2000. 14. Nguyen, L., N. Kelkar, and H. Takiar, “A Manufacturing Perspective of Wafer Level CSP,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 97–100, Las Vegas, NV, May 2000. 15. Topper, M., J. Auersperg, V. Glaw, K. Kaskoun, E. Prack, B. Keser, P. Coskina, D. Jager, D. Petter, O. Ehrmann, K. Samulewicz, C. Meinherz, S. Fehlberg, C. Karduck, and H. Reichl, “Fab Integrated Packaging (FIP): A New Concept for High Reliability Wafer-Level Chip Size Packaging,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 74–80, Las Vegas, NV, May 2000. 16. Ahn, M., D. Lee, and S. Kang, “Optimal Structure of Wafer Level Package for the Electrical Performance,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 530–534, Las Vegas, NV, May 2000. 17. Mirza, A. R., “One Micron Precision, Wafer-Level Aligned Bonding for Interconnect, MEMS and Packaging Applications,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 676–680, Las Vegas, NV, May 2000. 18. Simon, J., and H. Reichl, “Board Level Reliability of a Waferlevel CSP using Stacked Solder Spheres and a Solder Support Structure (S3),” IEEE Proceedings of Electronic Components & Technology Conference, pp. 81–86, Las Vegas, NV, May 2000. 19. Teutsch, T., T. Oppert, E. Zakel, E. Klusmann, H. Meyer, R. Schulz, and J. Schulze, “Wafer Level CSP using Low Cost Electroless Redistribution Layer,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 107–113, Las Vegas, NV, May 2000. 20. Tong, Q., B. Ma, E. Zhang, A. Savoca, L. Nguyen, C. Quentin, S. Luo, H. Li, L. Fan, and C. P. Wong, “Recent Advances on a Wafer-Level Flip Chip Packaging Process,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 101–106, Las Vegas, NV, May 2000. 21. Lau, J. H., C. Chang, and S. W. Lee, “Solder Joint Crack Propagation Analysis of Wafer-Level Chip Scale Package on Printed Circuit Board Assemblies,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 1360–1368, Las Vegas, NV, May 2000. 22. Lau, J. H., S. Pan, and C. Chang, “Nonlinear Fracture Mechanics Analysis of WaferLevel Chip Scale Package Solder Joints with Cracks,” Proceedings of IMAPS Microelectronics Conference, pp. 857–865, Boston, MA, September 2000.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
36
Chapter One
23. Lau, J. H., T. Chung, S. W. Lee, C. Chang, and C. Chen, “A Novel and Reliable WaferLevel Chip Scale Package (WLCSP),” Proceedings of SEMI Chip Scale International, pp. H 1–8, San Jose, CA, September 1999. 24. Jim, K. L., G. Faulkner, D. O’Brien, D. Edwards, and J. H. Lau, “Fabrication of Wafer Level Chip Scale Packaging for Optoelectronic Devices,” IEEE Proceedings of Electronic Components & Technology Conference, pp. 1145–1147, Las Vegas, NV, June 1999. 25. Lau, J. H., S. W. Lee, and C. Chang, “Solder Joint Reliability of Wafer Level Chip Scale Packages (WLCSP): A Time-Temperature-Dependent Creep Analysis,” ASME Trans., J. Electronic Packaging, 122(4): 311–316, December 2000. 26. Lau, J. H., “Cost Analysis: Solder Bumped Flip Chip Versus Wire Bonding,” IEEE Trans. Electronics Packaging Mfg., (23): 4–11, March 2000. 27. Lau, J. H., and C. Chang, “Overview of Microvia Technologies,” Circuit World, 26(2): 22–23, January 2000. 28. Lau, J. H., “Critical Issues of Wafer-Level Chip-Scale Package (WLCSP) with Emphasis on Cost Analysis and Solder Joint Reliability,” IEEE Proceedings of International Electronic Manufacturing Technology Symposium, pp. 33–46, San Jose, CA, October 2000. 29. Lau, J. H., S. Pan, and C. Chang, “Creep Analysis of Wafer Level Chip Scale Package (WLCSP) with 96.5Sn-3.5Ag and 100In Lead-Free Solder Joints and Microvia BuildUp Printed Circuit Board,” in Packaging of Electronic and Photonic Devices, ASME Book No. HO1217, pp. 79–89, November 2000. 30. Lau, J. H., S. Pan, and C. Chang, “A New Thermal-Fatigue Life Prediction Model for Wafer Level Chip Scale Package (WLCSP) Solder Joints,” in Packaging of Electronic and Photonic Devices, ASME Book No. HO1217, pp. 91–101, November 2000. 31. Gonzalez, C. G., R. A. Wessel, and S. A. Padlewski, “Epoxy-Based Aqueous Processable Photo Dielectric Dry Film and Conductive ViaPlug for PCB Build-Up and IC Packaging,” IEEE Trans. Adv. Packaging, 22(3):385–390, August 1999. 32. Singer, A. T., “Microvia Cost Modeling,” Proceedings from IPC Works, p. S-14-2, Washington, DC, October 1997. 33. Burgess, L. W., and P. D. Madden, “Blind Vias in SMD Pads,” Printed Circuit Fabrication, 21(1): 28–29, January 1998. 34. Castro, A., “Chip Carrier Package Constructions Made Easier with Dry Film Photo Dielectric,” Proceedings from IPC Works, p. S01-5-1, Washington, DC, October 1997. 35. Thorne, J., “Using New Interconnection Technologies to Reduce Substrate Cost,” IPC EXPO ’98, p. S-10, Long Beach, CA, April 1998. 36. Nargi-Toth, K., and P. Gandhi, “Manufacturing Methodologies for High Density Interconnect Structures (HDIS),” CSI Technical Symposium, pp. 63–70, San Jose, CA, September 1998. 37. Nargi-Toth, K., “ITRI Microvia Technology Roadshow,” IPC EXPO ’99, p. S17-1, Long Beach, CA, March 1999. 38. Numakura, D. K., S. E. Dean, D. J. McKenney, and J. A. DiPalermo, “Micro Hole Generation Processes for HDI Flex Circuit,” HDI EXPO ’99, pp. 443–450, Mesa, AZ, August 1999. 39. Noddin, D. B., E. Swenson, and Y. Sun, “Solid State UV-LASER Technology for the Manufacture of High Performance Organic Modules,” Proceedings of 48th Electronic Components and Technology Conference, pp. 822–827, Seattle, WA, May 1998. 40. Cable, A., “Improvements in High Speed Microvia Formation Using Solid State Nd:YAG UV Lasers,” IPC EXPO ’97, p. S-2, San Jose, CA, March 1997. 41. Owen, M., “Production Experiences with CO2 and UV YAG Drilling,” IPC EXPO ’97, p. S7-3, San Jose, CA, March 1997. 42. Tessier, T. G. and J. Aday, “Casting Light on Recent Advancements in Laser Based MCM-L Processing,” Proceedings 1995 International Conference on Multichip Modules, pp. 6–13, Denver, CO, April 1995. 43. Illyefalvi-Vitez, Z., M. Ruszinko, and J. Pinkola, “Recent Advancements in MCM-L Imaging and Via Generation by Laser Direct Writing,” Proceedings of 48th Electronic Components and Technology Conference, pp. 144–150, Seattle, WA, May 1998. 44. Moser, D, “Sights Set on Small Holes? How to Get There with Lasers,” Printed Circuit Fabrication, 20–22, February 1997.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
Introduction to Microvia and WLCSP Technologies
37
45. Owen, M., E. Roelants, and J. Van Puymbroeck, “Laser Drilling of Blind Holes in FR4/Glass,” Circuit World, 24(1): 45–49, 1997. 46. Contini, H. S., “Machining Lasers Find Niches by Solving Very Small Problems,” Photonics Spectra, 116–118, November 1997. 47. Illyefalvi-Vitez, Z. and J. Pinkola, “Application of Laser Engraving for the Fabrication of Fine Resolution Printed Wiring Laminates for MCM-Ls,” Proceedings of 47th Electronic Components and Technology Conference, pp. 502–510, San Jose, CA, May 1997. 48. Kobayashi, K., N. Katagiri, and S. Koyama, “Development of a Build Up Package with High Density of Circuits for High Pin Count Flip Chip Application,” IPC Expo 99, pp. S01–4, Long Beach, CA, March 1999. 49. Burgess, L. W., and F. Pauri, “Optimizing BGA to PCB Interconnections Using MultiDepth Laser Drilled Blind Vias-in-Pad,” Circuit World, 25(2): 31–34, 1999. 50. Raman, S., J. H. Jeong, S. J. Kim, B. Sun, and K. Park, “Laser (UV) Microvia Application in Cellular Technology,” IPC EXPO ’99, p. S17-6, Long Beach, CA, March 1999. 51. Schaeffer, R. D., “Laser Microvia Drilling: Recent Advances,” CircuiTree, 12, 38–44, 1998. 52. Petefish, W. G., D. B. Noddin, and D. A. Hanson, “High Density Organic Flip Chip Package Substrate Technology,” Proceedings of 48th Electronic Components and Technology Conference, pp. 1089–1097, Seattle, WA, May 1998. 53. Young, T. and F. Polakovic, “Thermal Reliability of Laser Ablated Microvias and Standard Through-Hole Technologies,” IPC Expo 99, pp. S17–2, Long Beach, CA, March 1999. 54. Gaku, M., H. Kimbara, N. Ikeguchi, and Y. Kato, “CO2 Laser Drilling Technology for Glass Fabrics Base Copper Clad Laminate,” IPC Expo 99, pp. S17–3, Long Beach, CA, March 1999. 55. Estes, W. E., T. R. Overcash, S. Padlewski, B. D. Neve, E. B. Murray, R. E. Anderson, R. C. Mason, and J. P. Lonneville, W. L. Hamilton and M. Periyasamy, “Photodielectric Dry Films for Ultra High Density Packaging,” SMI Proceedings, pp. 47–53, San Jose, CA, September 1997. 56. McDermott, B. J., and S. Tryzbiak, “The Practical Application of Photo-Defined Micro-Via Technology,” SMI Proceedings, pp. 199–207, San Jose, CA, September 1997. 57. Reboredo, L., “Microvias: A Challenge for Wet Processes,” IPC Expo 99, pp. S12–1, Long Beach, CA, March 1999. 58. Schmidt, W., “High Performance Microvia PWB and MCM Applications,” IPC Expo 99, pp. S17–5, Long Beach, CA, March 1999. 59. Ho, I., “What’s Up with SBU Technology?” Printed Circuit Fabrication, 64–68, March 1997. 60. Felten, J. J., and S. A. Padlewski, “Electrically Conductive Via Plug Material for PWB Applications,” IPC EXPO ’97, p. S6-6, San Jose, CA, March 1997. 61. Wessel, R. A., J. F. Henderson, J. J. Felten, S. Padlewski, M. A. Saltzberg, P. Charest, J. L. Parker, and P. T. Miscikowski, “A New Approach to Fill Conductive Vias in PCBs,” Printed Circuit Fabrication, 42–45, November 1997. 62. Nishii, T., S. Nakamura, T. Takenaka, and S. Nakatani, “Performance of Any Layer IVH Structure Multi-Layered Printed Wiring Board,” Proceedings of 1995 Japan IEMT Symposium, pp. 93–96, Omiya, Japan, December 1995. 63. Itagaki, M., K. Amami, Y. Tomura, S. Yuhaku, Y. Ishimaru, Y. Bessho, K. Eda, and T. Ishida, “Packaging Properties of ALIVH-CSP using SBB Flip-Chip Bonding Technology,” IEEE Trans. Adv. Packaging, 22(3): 366–371, August 1999. 64. Miyazawa, Y., T. Shirotsuki, H. Sugai, and Y. Yoneda, “Highly Accelerated Stress Test and Reliability Analysis for Build-up Circuits,” 1998 International Symposium on Microelectronics, pp. 430–434, San Diego, CA, November 1998. 65. Arike, S, K. Otsuka, N. Urasaki, A. Nakaso, K. Shibata, K. Kobayashi, K. Tsuyama, K. Suzuki, and H. Nakayama, “PWB using Mechanically Pre-drilled Metal Clad Film for IVH and Build-up PWB with Laser Via Hole for Semiconductor Package Substrate,” 1998 International Symposium on Microelectronics, pp. 425–429, San Diego, CA, November 1998.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Introduction to Microvia and WLCSP Technologies
38
Chapter One
66. Enomoto, R., M. Asai, and N. Hirose, “High Density MLB using Additive and Buildup Process,” 1998 International Symposium on Microelectronics, pp. 399–404, San Diego, CA, November 1998. 67. Tsukada, Y., and S. Tsuchida, “Surface Laminar Circuit, a Low Cost High Density Printed Circuit Board,” Proc. Surface Mount Int., 1: 537–542, August 1992. 68. Tsukada, Y., Y. Mashimoto, T. Nishio, and N. Mii, “Reliability and Stress Analysis of Encapsulated Flip Chip Joint on Epoxy Base Printed Circuit Board,” Proceedings of ASME/JSME Joint Conference on Electronic Packaging, vol. 2, pp. 827–835, San Jose, CA, September 1992. 69. Tsukada, Y., Y. Maeda, and K. Yamanaka, “A Novel Solution for MCM-L Utilizing Surface Laminar Circuit and Flip Chip Attach Technology,” Proceedings of 2nd International Conference on Multichip Modules,” pp. 252–259, Denver, CO, April 1993. 70. Tsukada, Y., “Solder Bumped Flip Chip Attach on SLC Board and Multichip Module,” in Chip on Board, Lau, J. H., ed., van Nostrand Reinhold, New York, pp. 410–443, 1994. 71. Segawa, K., “Build-Up PWB with Laser-Processed Via Holes ‘VIL’,” 1998 International Symposium on Microelectronics, 419–424, San Diego, CA, November 1998. 72. Kohl, P. A., C. S. Patel, and K. Martin, “Wafer-Level Batch Packaging and the Interface Between ICs and PWBs,” Chip Scale International 99, p. B-1, San Jose, CA, September 1999. 73. Maniwa, R., “Finer Micro-Via PWB by Laser and Additive Process,” 1998 International Symposium on Microelectronics, 413–418, San Diego, CA, November 1998. 74. Fukuoka, Y., T. Oguma, and Y. Tahara, “New High Density Substrates with Buried Bump Interconnection Technology (B2it)—Design Features of Electrical and Thermal Performances with the Actual Applications,” 1998 International Symposium on Microelectronics, pp. 405–412, San Diego, CA, November 1998. 75. Jimarez, M., L. Li, C. Tytran, C. Loveland, and J. Obrzut, “Technical Evaluation of a Near Chip Scale Size Flip Chip/Plastic Ball Grid Array Package,” Proceeding of IEEE ECTC, pp. 495–502, Seattle, WA, June 1998. 76. Mawer, A., K. Simmons, T. Burnette, and B. Oyler, “Assembly and Interconnect Reliability of BGA Assembled onto Blind Micro and Through-Hole Drilled Via in Pad,” Proceedings of SMI Conference, pp. 21–28, San Jose, CA, August 1998. 77. IPC-2141, Controlled Impedance Circuit Boards and High-Speed Logic Design, April 1996. 78. Wadel, B., Transmission Line Design Handbook, Artech House, 1991.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Source: Microvias
Chapter
2 Conventional Printed Circuit Board Technologies
2.1 Introduction Modern electronic packaging has become very complex. Interconnections are pushed more into lower levels of packaging. The choice of which packaging technology to use is governed by many factors: cost, electrical requirements, thermal requirements, density requirements, and so on. Material also plays a very important role. All things considered, PCBs play very important roles in electronic packaging.1 Since the invention of printed circuit technology by Dr. Paul Eisner in 1936, several methods and processes have been developed for manufacturing PCBs of various types. Most of these have not changed significantly over the years. However, some specific trends continue to exert major influences on the types of PCBs required and the processes that create them: 1. Computers and portable telecommunications equipment require higher-frequency circuits, boards, and materials, and also use more functional components that generate considerable amounts of heat that need to be extracted. 2. Consumer products have incorporated digital products into their design, requiring more functionality at ever lower total cost. 3. Products for all uses continue to get smaller and more functional, driving the total circuit package itself to become more dense, causing the PCBs to evolve to meet these needs.
39
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
40
Chapter Two
These will be discussed in this chapter, along with the traditional board structures and processes. The terms printed circuit board, PCB, and board will be used synonymously. Also, the words laminate, substrate, and panel will be used interchangeably.
2.2 Types of Printed Circuit Boards 2.2.1 Basic PCB classifications
PCBs may be classified in many different ways according to their various attributes. One fundamental structure common to all of them is that they must provide electrical conductor paths that interconnect components to be mounted on them. There are two basic ways to form these conductors: 1. Subtractive. In the subtractive process, the unwanted portion of the copper foil on the base substrate is etched away, leaving the desired conductor pattern in place. 2. Additive. In the additive process, formation of the conductor pattern is accomplished by adding copper to a bare (no copper foil) substrate in the pattern and places desired. This can be done by plating copper, screening conductive paste, or laying down insulating wire onto the substrate on the predetermined conductor paths. The PCB classifications given in Fig. 2.1 take into consideration all these factors, i.e., fabrication processes as well as substrate materials. The use of Fig. 2.1 is as follows: ■
Column 1 shows the classification of PCBs by the nature of the substrate.
■
Column 2 shows the classification of PCBs by the way the conductor pattern is imaged.
■
Column 3 shows the classification of PCBs by their physical nature.
■
Column 4 shows the classification of PCBs by the method of conductor formation.
■
Column 5 shows the classification of PCBs by the number of conductor layers.
■
Column 6 shows the classification of PCBs by the existence or absence of PTHs.
■
Column 7 shows the classification of PCBs by production method.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.1
41
Classification of printed circuit boards.
2.2.2 Other classifications of PCBs
One of the major issues that has arisen with the ever higher speed and functionality of components used in computers and telecommunications is the availability of materials for the PCB substrate that are compatible with these product and process needs. This includes the stresses on substrate material created by more and longer exposure to soldering temperatures during the assembly process, as well as the need to match the coefficient of thermal expansion for components and substrate. The resultant search has found new materials, both organic and nonorganic based.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
42
Chapter Two
Organic substrates consist of layers of paper impregnated with phenolic resin or layers of woven or nonwoven glass cloth impregnated with epoxy resin, polyimide, cyanate ester, BT resin, etc. The usage of these substrates depends on the physical characteristics required by the application of the PCB, such as operating temperature, frequency, or mechanical strength. Nonorganic substrates consist mainly of ceramic and metallic materials such as aluminum, soft iron, and copperinvar-copper. The usage of these substrates is usually dictated by the need for heat dissipation, except for the case of soft iron, which provides the flux path for flexible disk motor drives. PCBs may be classified into two other categories, graphical and discrete-wire boards, based on the way they are manufactured. A graphical PCB is the standard PCB and the type that is usually thought of when PCBs are discussed. In this case, the image of the master circuit pattern is formed photographically on a photosensitive material, such as treated glass plate or plastic film. The image is then transferred to the circuit board by screening or photoprinting the artwork generated from the master. Due to the speed and economy of making master artwork by laser plotters, this master can also be the working artwork. Discrete-wire boards do not involve an imaging process for the formation of signal conductors. Rather, conductors are formed directly onto the wiring board with insulated copper wire. Wire-wrap® and Multiwire® are the best known discrete-wire interconnection technologies. Because of the allowance of wire crossings, a single layer of wiring can match multiple conductor layers in the graphically produced boards, thus offering very high wiring density. However, the wiring process is sequential in nature and the productivity of discrete-wiring technology is not suitable for mass production. Despite this weakness, discrete-wiring boards are in use for some very high-density packaging applications. Another class of boards is made up of the rigid and flexible PCBs. Whereas boards are made of a variety of materials, flexible boards generally are made of polyester and polyimide bases. RigiFlex boards, a combination of rigid and flexible boards bonded together, have gained wide use in electronic packaging (see Fig. 2.2). Most RigiFlex boards are three-dimensional structures that have flexible parts connecting the rigid boards, which usually support components; this packaging is thus volumetrically efficient. 2.2.3 Graphically produced boards
The majority of boards produced in the world are graphically produced. There are three alternative types: single-sided boards, double-sided boards, and multilayer boards.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.2
43
RigiFlex printed circuit board.
2.2.3.1 Single-sided boards (SSBs). Single-sided boards have circuitry on only one side of the board and are often referred to as print-and-etch boards because the etch resist is usually printed on by screen-printing techniques and the conductor pattern is then formed by chemically etching the exposed, and unwanted, copper foil. This method of board fabrication is generally used for low-cost, highvolume, and relatively low-functionality boards. In the Far East, for example, the majority of SSBs are made of paper-based substrates for lowest cost, with the most popular grade of paper-based laminate being
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
44
Chapter Two
XPC-FR, which is a flame-retardant phenolic material that is also highly punchable. In Europe, FR-2 grade paper laminate is the most popular substrate for SSBs because it emits less odor than XPC-FR when placed in high-voltage, high-temperature environments, such as inside a television set chassis. In the United States, CEM-1 material, which is a composite of paper and glass impregnated with epoxy resin, is the most popular substrate for SSBs. While not as low-cost as XPC-FR or FR-2, CEM-1 has gained popularity because of its mechanical strength and also because of the relative unavailability of paper phenolic laminates. 2.2.3.2 Double-sided boards (DBs). By definition, double-sided boards have circuitry on both sides. They can be classified into two categories: with and without through-hole metallization. The category of throughhole metallization can be further broken into two types: plated throughhole (PTH) and silver through-hole (STH).2 Metallization of holes by copper plating has been practiced since the mid-1950s. Because PCB substrate is an insulating material, and therefore nonconductive, holes must be metallized first before subsequent copper plating can take place. The usual metallization procedure is to catalyze the holes with palladium catalyst followed by electroless copper plating. Then, thicker plating is done by means of galvanic plating. Alternately, electroless plating can be used to plate all the way to the desired thickness, which is called additive plating. The biggest change in the manufacturing process of double-sided PTH boards, and also of multilayer boards (MLBs), is the use of direct metallization technologies. In this case the electroless copper process is eliminated. The hole wall is made conductive by palladium catalyst, carbon, or polymer conductive film, and then copper is deposited by galvanic plating. The elimination of electroless copper, in turn, allows the elimination of environmentally hazardous chemicals, such as formaldehyde and EDTA, which are two main components of electroless copper-plating solutions. STH boards are usually made of paper phenolic materials or composite epoxy paper and glass materials, such as CE-1 or CE-3. After double-sided copper-clad materials are etched to form conductor patterns on both sides of the panel, holes are formed by drilling. Then the panel is screened with silver-filled conductive paste. (Instead of silver, copper paste can also be used.) Since STH boards have a relatively high electrical resistance compared with PTH boards, the application of STH boards is limited. However, because of their economic advantage (the cost of STH boards is usually one-half to two-thirds that of functionally equivalent PTH boards), their application has spread to high-volume, low-cost products such as audio equipment, floppy disk controllers, car radios, remote controls, etc.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
45
2.2.3.3 Multilayer boards (MLBs). By definition, MLBs have three or more circuit layers (see Fig. 2.3). Main applications of MLBs used to be confined to sophisticated industrial electronic products. Now, however, they are the mainstream of all electronic devices, including consumer products such as portable video cameras, cellular phones, and audio discs. As personal computers and workstations become more powerful, mainframe computers and supercomputers are being replaced in many applications by these smaller machines. As a result, the use of highly sophisticated MLBs, which have layer counts over 70, is being reduced, but the technology to produce them is proven. At the other end of the layer-count spectrum, thin and high-density MLBs with layer counts between four and eight are mainstream. The drive toward thinner MLBs will continue and is made possible by the continuing concurrent advancement of materials and equipment to handle thin core materials. As PCBs have had to address the issues of higher speed, higher density, and the rise of surface-mount components that use both sides, the need to communicate between layers has increased dramatically. At the same time, the space available for vias has decreased, causing a continuing trend toward smaller holes, more holes on the board, and the decline of the use of holes that penetrate the entire board, which use space on all layers. As a result, the use of buried and blind vias has become a standard part of multilayer board technology, driven by the need for this increased package density (Fig. 2.3). One of the immediate issues that arise from these trends is the problems of drilling and the associated cost of this fabrication step. Printed circuit boards, which once were stacked three high on a drilling machine, must be drilled individually, and the number of holes per board has risen to accommodate the need for vias. This has caused a major problem for fabricators, who find that a lack of drilling capacity is creating a big demand on funds for additional machines, while
Figure 2.3
Cross section of multilayer board with buried via
holes.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
46
Chapter Two
the cost of drilling continues to increase dramatically. Therefore, alternate methods for creating vias are being developed. These pressures will be ongoing, and therefore the process listed here, or some equivalent, will undoubtedly become more important as the drive toward miniaturization continues and drilling individual holes becomes less and less practical.
2.3 Base Materials 2.3.1 Copper-clad laminates
It is important to understand the types of copper-clad laminates that are available, how they are made, where they are used, and the advantages and disadvantages of each before selecting the material most suitable for the intended application. Many types of copper-clad materials are available (see Fig. 2.4). The copper-clad laminates most widely used in the manufacture of printed circuit boards, however, are FR-2, CEM-1, CEM-3, FR-4, FR-5, and GI. These are the materials that are primarily discussed in this section. The FR-2 laminates are composed of multiple plies of paper that have been impregnated with a flame-retardant phenolic resin. The major advantages of FR-2 laminates are their relative low cost and their good electrical and punching qualities. FR-2 is typically used in
Figure 2.4
PCB designations and materials.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
47
applications where tight dimensional stability is not required, such as in radios, calculators, toys, and television games. FR-3, the other all-paper-base laminate, is also made of multiple plies of paper that have been impregnated with an epoxy-resin binder. The FR-3 laminate has electrical and physical properties that are higher than those of the FR-2 but lower than those of epoxy laminates that have woven glass cloth as a reinforcement. FR-3 is used to manufacture printed circuits used in consumer products, computers, television sets, and communication equipment. CEM-1 is a composite material that has a paper core impregnated with epoxy resin. Woven glass cloth impregnated with the same resin covers the two surfaces. This construction allows the material to have punching properties similar to those of FR-2 and FR-3, with electrical and physical properties approaching those of FR-4. CEM-1 is used in smoke detectors, television sets, calculators, and automobiles as well as in industrial electronics. CEM-3, a composite of dissimilar core material, uses an epoxy-resinimpregnated nonwoven fiberglass core with epoxy-resin-impregnated woven glass cloth surface sheets. It is higher in cost than CEM-1, but it is more suitable for plated through-holes. CEM-3 is used in applications such as home computers, automobiles, and home entertainment products. FR-4 laminates are constructed on multiple plies of epoxy-resinimpregnated woven glass cloth. It is the most widely used material in the printed circuit board industry because its properties satisfy the electrical and mechanical needs of most applications. Its excellent electrical, physical, and thermal properties make it a well-suited material for high-technology applications. It is used in aerospace, communications, computers and peripherals, industrial controls, and automotive applications. FR-5 laminates are composed of multiple plies of woven glass cloth impregnated with mostly polyfunctional epoxy resin. The glass transition temperature Tg is typically 150 to 160°C, as compared with FR-4, which has a glass transition temperature of 125 to 135°C. FR-5 is used where higher heat resistance is needed than is attainable with FR-4, but not where the very high thermal properties of GI-type materials are needed. GI-type materials are composed of multiple plies of woven glass cloth impregnated with a polyimide resin. The materials have a glass transition temperature in excess of 200°C, which virtually eliminates “drill smear” caused by heat during the drilling process. It also exhibits excellent mechanical properties and z-axis dimensional stability at high temperatures. GI materials have a lower interlaminar bond strength
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
48
Chapter Two
than the epoxy systems; therefore, care should be taken during drilling and routing. 2.3.2 Considerations in glass transition temperature Tg
Tg has become a measure of how well a laminate resin system resists softening from heat. When the Tg temperature is reached, the resin changes from its “glassy” state and causes changes in the laminate’s properties. Tg is not a measure of the resin’s melting point, but rather a point at which molecular bonds begin to weaken enough to cause a change in physical properties (dimensional stability, flexural strength, etc.). Its value is determined by the intersection of the two slopes of the temperature-property-change curve (Fig. 2.5a). FR-4 epoxy exhibits a Tg of 125 to 135°C and polyimide 260 to 300°C. Although the Tg value is a measure of the toughness of a material under heating, it is not meant for comparison purposes once the Tg
TE21
Property change
Tg Temperature
(a)
Property change
Resin x Resin y Tg(x)
Tg(y)
Temperature
(b)
(a) Determination of glass transition temperature Tg. (b) General features of Tg. Figure 2.5
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
49
is exceeded. For example, materials with a higher Tg are desirable because they maintain their stability over a wider temperature range up to the Tg. However, once the Tg is exceeded, the material properties of a high-Tg resin could change much more rapidly than those of a material with a low Tg. At a higher temperature, the lower-Tg material may often exhibit superior properties (Fig. 2.5b). 2.3.3 Lamination process 2.3.3.1 Material preparation. The base raw material—paper, glass matte, woven glass cloth, quartz, or Kevlar®—is impregnated or coated with resin. The resin is then polymerized to a point suitable for storage and final pressing. A machine called a treater or coater is used for treating the material. First the material passes through a dip pan of resin, where it is impregnated, and then through a set of metering rollers (squeeze rollers) and a drying oven. The oven is air-circulating or infrared and can be up to 120 ft long. Most of the volatiles such as solvents in the resin are driven off in the oven, and the resin is polymerized to what is called a B-stage. This semicured material is also known as prepreg. The prepreg is dry and nontacky. The treater illustrated in Fig. 2.6 is a vertical treater that runs principally woven glass cloth; horizontal treaters impregnate mainly paper and glass matte. Rigid process control is applied during treating so that the ratio of resin to base material, the final thickness of the prepreg, and the degree of resin polymerization can be monitored. Beta-ray gauges may compare the raw material with the final semicured product and automatically adjust the metering rollers above the resin dip pan so that the proper
Figure 2.6
Features of the vertical tower processing system.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
50
Chapter Two
ratio of resin to base material is maintained. The degree of polymerization of the resin is controlled by the treater air temperature, the air velocity, and the speed at which the material passes through the treater. The prepreg material is usually stored in an area where the temperature and humidity are controlled below 21°C and 35 percent relative humidity (RH), respectively, until the time of the pressing operation. Each roll or stack of prepreg is tagged with the processing date and the test results for resin content, gel time, resin flow, cured thickness, and volatile content. 2.3.3.2 Copper inspection. Besides the base material and resin, the other principal component of copper-clad laminates is copper foil. Today, almost all copper is electrodeposited rather than rolled. Each roll of copper is inspected by the laminator for visual surface quality and pinholes, and a sample is taken for trial pressing. The trial pressing sample is tested for copper peel strength, solder blister resistance, copper oxidation after heat exposure, and general surface quality. The side of the foil to be pressed against the prepreg is treated with an alloy to improve adhesion of the copper to the laminate. The alloy is a proprietary coating, usually of zinc or brass, in a controlled ratio to enhance the chemical bond between the copper and the resin. 2.3.3.3 Laminate buildup. Most laminators build up their sheets in clean room facilities with filtered air-conditioned systems to control the temperature and humidity as well as to keep dust particles away from the copper and prepreg during buildup. Electrostatic attraction of dust particles to the treated material and copper before pressing is a source of contamination in the laminate and a source of pits and dents on the copper surface of the finished laminate. During the buildup operation, the copper foil is first laid against a large polished stainless steel press plate. Then a number of sheets of prepreg are laid on top of the copper. The number of layers depends on the desired thickness of the laminate and the characteristics of the prepreg material. Some of the art of laminating comes in balancing all of these variables to produce a final dense material to relatively close tolerances. The final sheet of copper foil is placed on top of the prepreg if the material is to have copper on both sides. If copper is desired on only one side of the laminate, a release film such as Tedlar® replaces one of the sheets of copper. 2.3.3.4 Laminate pressing. The press plates, with the material, are removed from the buildup room and stacked in a large, multiopening press. Several sheets are pressed into each press opening, with typical presses being capable of molding 80 sheets 36 × 48 in. to 250 sheets 48 × 144 in., 1⁄16 in. thick. The presses, which are hydraulic, are capable of developing pressure in excess of 1000 lb/in2. Steam is a typical heat source. It is released into the press platens until the platens reach the Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
51
uniform laminating temperature. The packs or books of material are then loaded into the press, and the desired pressure is applied so that the material is cured into a final homogeneous sheet. To ensure that all of the sheets in the pack or book receive the desired state of cure, thermocouples are placed in several sheets in the press. A timer automatically records time against a preset cure cycle. When the desired stage of cure is achieved, the steam is automatically cut off and cold water is pumped through the press platens until the material reaches approximately 27°C. The material is then removed from the press, and the edges are trimmed from the sheet to remove irregular resin flow areas. 2.3.3.5 Laminating quality control system. Statistical process control methods are used to verify that each step in the manufacturing process is controlled. Figure 2.7 outlines laminate traceability. Each press load is tested according to the appropriate sampling plan to ensure that the material will meet customer requirements. Each sheet is then identified as to manufacturer, appropriate specification, and load or lot number. Most manufacturers retain samples of material from each load for at least 1 year to enable them to effectively check any processing problems or questions that may result from the use of that lot in the field. Periodically, laminators are required to run a complete set of physical and electrical tests as set forth by the National Electrical Manufacturers Association (NEMA) or MIL-P-13949. 2.3.4 Grades and specifications
The grades and specifications of some standard laminates are presented in Tables 2.1 to 2.3. The most common method of designating copper-clad materials is described in MIL-P-13949 and illustrated in Fig. 2.8. As an example, GFN-0620-CN/CI-A-2-A means no coloring in flame-retardant glass-epoxy laminate, 0.062 in thick, 1⁄2-oz/ft2 copper, drum side out, on one side, and 1-oz/ft2 copper, drum side out, on the other side, Grade A pits and dents, Class 2 thickness tolerance, and Class A warp and twist.
Figure 2.7
Flow chart for laminate quality control.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
GP
GH
GI
FR-5
None
None
FR-6
G-11
None
CEM-3
GE
None
CEM-1
GF
PX
FR-3
FR-4
None
FR-2
G-10
None
XXXPC
Polyimide
Epoxy
Epoxy
Epoxy
Epoxy
Polyester
Epoxy
Epoxy
Epoxy
Phenolic
Phenolic
Glass
Glass
Glass
Glass
Glass
Glass matte
Glass matte
Paper-glass composite
Paper
Paper
Paper
Base
Military designation MIL-P-13949F
NEMA grade
Resin system
Standard Materials for Printed Circuit Boards
TABLE 2.1
Color
Translucent dark brown
Translucent
Translucent
Translucent
Translucent
Opaque white
Translucent
Opaque tan
Opaque cream
Opaque brown
Opaque brown
Description
Polyimide resin, glass laminate with high continuous operating temperature and high property retention at temperature, low z-dimensional expansion
High-temperature epoxy-glass with flame-resistant resin system with strength and electrical retention at elevated temperatures
High-temperature epoxy-glass with strength and electrical retention at elevated temperatures
Epoxy-glass with self-extinguishing resin system
Epoxy-glass, general purpose
Polyester, random glass fiber, flame-resistant, designed for low-capacitance or high-impact applications
Epoxy resin nonwoven glass core with woven glass surfaces, self-extinguishing, punchable with properties similar to FR-4
Epoxy resin paper core with glass on the laminate surface, self-extinguishing, economic fabrication of paper base, mechanical characteristics of glass
Epoxy resin, paper base with flame-resistant resin system, cold punching, and high insulation resistance
Phenolic paper, punchable, with flame-resistant (self-extinguishing) resin system
Phenolic paper with punchability at or above room temperature Conventional Printed Circuit Board Technologies
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
52
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
TABLE 2.2
53
Materials for High-Frequency Applications
NEMA grade
Military Designation MIL-P13949
GT
GX
Resin system
Base
Color
Description
GT
TFE
Glass
Opaque brown
Glass fabric base, PTFE (Teflon) resin, controlled dielectric constant
GX
TFE
Glass
Opaque brown
Glass fabric base, PTFE (Teflon) resin dielectric constant with closer controlled limits than GT
Polystyrene
Glass
Opaque white
Polystyrene cast-resin base for low-dissipation-factor applications
Cross-linked polystyrene
Glass
Opaque white
Polyethylene cast base, radiation cross-linked for low dissipation factor
The conditioning designations used to describe the environment in which tests were run are as follows: ■
Condition A. As received; no special conditioning
■
Condition C. Humidity conditioning
■
Condition D. Immersion conditioning in distilled water
■
Condition E. Temperature conditioning
■
Condition T. Test conditioning
Conditioning procedures are designated in accordance with the following: ■
First, a capital letter indicating the general condition of the specimen to be tested, i.e., as received or conditioned to humidity, immersion, or temperature.
■
A number indicating the duration of the conditioning, in hours, follows.
2.3.5 Mechanical properties of laminates
The principal characteristics usually required in the mechanical design of printed boards are outlined here. If a specific test is required, the test is listed under a particular heading. Whenever they are available, the minimum standards set forth in MIL-P-13949 or NEMA standards for industrial laminates are used.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Military designation MIL-P-13949
None None None None
None None None None None
None
None None None
None
XXXPC FR-2 FR-3 FR-4
XXXPC FR-2 FR-3 FR-4 CEM-1
CEM-3
FR-2 FR-3 FR-4
FR-4
Epoxy
Phenolic Phenolic Epoxy
Epoxy
Phenolic Phenolic Phenolic Epoxy Epoxy
Phenolic Phenolic Phenolic Epoxy
Resin system Base
Color
Opaque brown Opaque brown Opaque brown Translucent
Adhesives
Glass
Translucent
Swell and etch
Paper Paper Glass, glasspaper composite
Sacrificial aluminum-clad
Opaque brown Opaque brown Opaque brown Translucent Opaque tan, blue, white Translucent
Seeded and coated Paper Paper Paper Glass Paper-glass composite Glass-matte composite
Paper Paper Paper Glass
Materials for Additive Circuit Processing
NEMA grade
TABLE 2.3
This laminate is used in the commercially available swell-and-etch additive process. The epoxy-glass laminate has a 0.0015-in.thick resin-rich surface and a specially designed surface for swell-and-etch chemicals.
These laminates are the patented sacrificial additive process. They are clad on two sides with a specially anodized aluminum foil. The sacrificial aluminum cladding makes the laminate surface acceptable for the additive process.
These laminates are used in the patented seeded and coated processes. They are seeded with a small percentage of the catalytic seeding agent dispersed throughout the resin system and are coated with a catalyzed adhesive.
These laminates are designed for use with additive processes using adhesive bonding techniques.
Description
Conventional Printed Circuit Board Technologies
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
54
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.8
55
Designation of Cu-clad laminates.
2.3.5.1 Thickness tolerance. Nominal thicknesses and tolerances should be specified per MIL-P-13949. At least 90 percent of the area of a sheet should be within the tolerance given, and at no point should the thickness vary from the nominal by a value greater than 125 percent of the specified tolerance. Cut sheets less than 18 × 18 in. should meet the applicable thickness tolerance in 100 percent of the area of the sheet. Class of tolerance is as specified in the type designation. For nominal thicknesses not shown in this table, the tolerance for the next greater thickness shown applies. The nominal thicknesses include metal foil except in the case of microwave materials, which are without foil. (See Table 2.4.) 2.3.5.2
Flexural strength. Method: ASTM D 790. Unit of value: lb/in2.
This test is measure of the load that a beam will stand without fracture when supported at the ends and loaded in the center, as shown in Fig. 2.9. (See Table 2.5.) 2.3.5.3 Coefficient of thermal expansion (CTE). Method: ASTM D 696 (at 130°F). Unit of value: in./in./°F. The coefficient of thermal expansion (Table 2.6) is the change in length per unit of length per degree change in temperature. The coefficient may vary in different temperature ranges, so the temperature range must be specified.
TABLE 2.4
Nominal Thickness and Tolerance for Laminates (MIL-P-13949F) Class 1
Thickness (in. × 10−3)
PX paper base only
Glassreinforced
Class 2 glassreinforced
Class 3 glassreinforced
Class 4 for microwave application
0010 to 0045 0046 to 0065 0066 to 0120 0121 to 0199 0200 to 0309 0310 to 0409 0410 to 0659 0660 to 1009 1010 to 1409 1410 to 2400
— — — — — ⫾0045 ⫾0060 ⫾0075 ⫾0090 ⫾0120
⫾0010 ⫾0015 ⫾0020 ⫾0025 ⫾0030 ⫾0065 ⫾0075 ⫾0090 ⫾0120 ⫾0220
⫾00075 ⫾0010 ⫾0015 ⫾0020 ⫾0025 ⫾0040 ⫾0050 ⫾0070 ⫾0090 ⫾0120
⫾0005 ⫾00075 ⫾0010 ⫾0015 ⫾0020 ⫾0030 ⫾0030 ⫾0040 ⫾0050 ⫾0060
— — — — — ⫾002 ⫾002 ⫾002 ⫾0035 ⫾0040
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
56
Chapter Two
Figure 2.9
Flexural strength test.
2.3.5.4 Water absorption. Unit of value: Percent water absorption is the ratio of weight of water absorbed by the material to the weight of the dry material. (See Table 2.7.) 2.3.5.5 Flammability. According to Underwriters Laboratories, materials tested for flammability are classified 94V-0, 94V-1, and 94V-2. For material flame ratings, see Table 2.8. Definitions of those classifications, as tested by the Underwriters Laboratories flammability procedure, are outlined as follows. ■
94V-0. Specimens must extinguish within 10 s after each flame application and a total combustion of less than 50 s after 10 flame applications. No samples are to drip flaming particles or have glowing combustion lasting beyond 30 s after the second flame test.
■
94V-1. Specimens must extinguish within 30 s after each flame application and a total combustion of less than 250 s after 10 flame applications. No samples are to drip flaming particles or have glowing combustion lasting beyond 60 s after the second flame test.
■
94V-2. Specimens must extinguish within 30 s after each flame application and a total combustion of less than 250 s after 10 flame applications. Samples may drip flame particles, burning briefly, and no specimen will have glowing combustion beyond 60 s after the second flame test.
TABLE 2.5
Flexural Strength (Condition A, Minimum Average psi) Material
Lengthwise
Crosswise
XXXPC FR-2 FR-3 FR-4 FR-5 FR-6 G-10 G-11 CEM-1 CEM-3 GT GX GI
12,000 12,000 20,000 60,000 60,000 15,000 60,000 60,000 35,000 40,000 15,000 15,000 50,000
10,500 10,500 16,000 50,000 50,000 15,000 50,000 50,000 28,000 32,000 10,000 10,000 40,000
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
TABLE 2.6
57
Coefficient of Thermal Expansion
(CTE) Coefficient, × 10−5 Material
Lengthwise
Crosswise
Ordinary applications XXXP XXPC FR-2 FR-3 CEM-1 CEM-3 FR-6 G-10 FR-4 G-11 FR-5 GI
1.2 1.2 1.2 1.3 1.1 1.0 1.0 1.0 1.0 1.0 1.0 1.0
1.7 1.7 2.5 2.5 1.7 1.5 1.0 1.5 1.5 1.5 1.5 1.2
High-frequency applications GT GX Polystyrene Cross-linked polystyrene
TABLE 2.7
1.0 1.0 7.0 5.7
2.5 2.5 7.0 5.7
Water Absorption (Condition D 24/23)
Material
⁄32 in.
1
⁄16 in.
1
⁄32 in.
3
Ordinary applications XXXP XXXPC FR-2 FR-3 CEM-1 CEM-3 FR-6 G-10 FR-4 G-11 FR-5 GI
1.3 1.3 1.3 1.0 0.50 0.50 0.50 0.50 0.50 0.50
1.0 0.75 0.75 0.65 0.30 0.25 0.40 0.25 0.25 0.25 0.25 1.0
0.85 0.65 0.65 0.60 0.25 0.20
0.10 0.10 0.05 0.01
0.09 0.09
0.20 0.20 0.20 0.20
High-frequency applications GT GX Polystyrene Cross-linked polystyrene
0.20 0.20
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
58
Chapter Two
TABLE 2.8
Grade XXXPC FR-2 FR-3 CEM-1 CEM-3
■
Flammability Classifications UL classification
Grade
UL classification
94HB 94V-1 94V-0 94V-0 94V-0
G-10 FR-4 G-11 FR-5 FR-6
94HB 94V-0 94HB 94V-0 94V-0
94HB. Specimens are to be horizontal and have a burning rate less than 1.5 in./min over a 3.0-in. span. Sample must cease to burn before the flame reaches the 4-in. mark.
2.3.6 Electrical properties of laminates 2.3.6.1 Surface resistivity. The effect of humidity on the surface resistance of glass-epoxy was measured by using the American Society for Testing Materials (ASTM) three-electrode circular pattern, starting with 97.5 percent RH at 40°C and decreasing the humidity to 64 percent. The results, shown in Fig. 2.10, indicate that the surface resistivity decreases logarithmically with an increase in humidity at approximately the rate of 1 decade per 20 percent humidity change. 2.3.6.2 Dielectric strength. (Perpendicular to the laminations at 23°C.) Method: ASTM D 149. Unit of value: V/mil. Dielectric strength is the ability of an insulation material to resist the passage of a disruptive discharge produced by an electric stress.3 A disruptive discharge is measured by applying 60-Hz voltage through the thickness of the laminate, as shown in Fig. 2.11. All the tests are run under oil. In the shorttime test the applied voltage is increased at a uniform rate of 0.5 kV/s. In the step-by-step test, the initial voltage is 50 percent of the shorttime breakdown voltage; thus, the voltage is increased in increments according to a predetermined schedule of 1-min intervals. The test val-
Figure 2.10
Surface resistivity vs. relative humidity.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.11
59
Dielectric strength test.
ues for dielectric strength vary with the thickness of the material, the form and size of electrodes, the time of application of the voltage, the temperature, the frequency and wave shape of the voltage, and the surrounding medium. Step-by-step data for 1⁄16-in.-thick material are as shown in Table 2.9. 2.3.6.3 Dielectric breakdown. (Parallel to the laminations at 23°C.) Method: ASTM D 149. Unit of value: kV. Condition D 48/50. Dielectric breakdown is the disruptive discharge measured between two electrodes (Pratt and Whitney No. 3 taper pins) inserted in the laminate on 1-in. centers perpendicular to the laminations.4 All tests are run under oil. The short-time and step-by-step tests are performed as in the test for dielectric strength perpendicular to laminations. Step-by-step data on 1⁄16-in.-thick material are given in Table 2.10. 2.3.6.4 Dielectric constant (permitivity). Method: ASTM D 150. Unit of value: dimensionless. Dielectric constant is the ratio of the capacitance of a capacitor with a given dielectric to the capacitance of the same capacitor with air as a dielectric, as illustrated in Fig. 2.12. The dielectric constant is a measure of the ability of an insulating material to store electrostatic energy. It is calculated from the capacitance as read TABLE 2.9
Material XXXP FR-2 FR-3 CEM-1 CEM-3
TABLE 2.10
Dielectric Strength Data V/mil
Material
V/mil
740 740 550 500 500
G-10 G-11 FR-4 FR-5 GI
510 600 500 500 750
Dielectric Breakdown Data
Material
kV
Material
kV
XXXPC FR-2 FR-3 FR-6 CEM-1 CEM-3
15 15 30 30 40 40
G-10 FR-4 G-11 FR-5 GT GX
40 40 40 40 20 20
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
60
Chapter Two
Dielectric constant test.
Figure 2.12
on a capacitance bridge, the thickness of the specimen, and the area of the electrodes. It varies with temperature, humidity, and frequency. (See Table 2.11.) 2.3.6.5 Dissipation factor. (Average at 1 MHz.) Method: ASTM D 150. (See Fig. 2.13.) Unit of value: dimensionless. In an insulating material, the dissipation factor is the ratio of the total power loss, in watts, in the material to the product of the voltage and current in a capacitor in which the material is a dielectric. It varies over a frequency range. (See Tables 2.12 and 2.13.)
2.4 Imaging/Drilling/Plating/Etching 2.4.1 Imaging processes
The imaging process comprises several sequential steps that together allow for the metal interconnect pattern to be formed on a bare substrate. The steps themselves are interactive and it is a balance between them that allows for the reproduction of a master pattern into a metal TABLE 2.11
Materials
Permittivity Permittivity at 1 MHz (Condition D 24/23)
Ordinary applications XXXPC FR-2 FR-3 CEM-1 CEM-3 FR-6 G-10 FR-4 G-11 FR-5 GI
4.1 4.5 4.3 4.4 4.6 4.1 4.6 4.6 4.5 4.3 4.8 High-frequency applications
GT GX Polystyrene Cross-linked polystyrene
2.8 2.8 2.5 2.6
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.13
61
Dissipation factor test.
pattern with high fidelity. The success of the steps in the sequence is dependent on the materials or chemicals used, but also to a large extent on the equipment utilized. Thus, again there is a balance of various factors needed in order to obtain a stable, reproducible, and highyield/low-cost process. The details of the chemistry and the equipment used to perform it will be outlined, and as often as possible the tradeoffs of various choices will be highlighted so that both the inexperienced process engineers and the designers and procurers of PCBs who need an overview of the process considerations will be able to proceed in their work to obtain a manufacturable product. The process sequence for imaging is given in Fig. 2.14, where the resulting pattern is used for either subtractive or additive metal pattern transfer. The details of these processes are given in the subsequent chapters. In a generic sense the process involves the coating of a polymeric material onto the substrate of interest, patterning the TABLE 2.12
Dissipation Factors Dissipation factor at 1 MHz
Materials
Condition A
Condition D 24/23
Ordinary applications XXXP XXXPC FR-2 FR-3 CEM-1 CEM-3 FR-6 G-10 FR-4 G-11 FR-5 GI
0.028 0.028 0.024 0.024 0.027 0.020 0.020 0.018 0.018 0.019 0.019 0.020
0.03 0.03 0.026 0.026 0.028 0.022 0.028 0.019 0.020 0.020 0.028 0.030
High-frequency applications GT GX Polystyrene Cross-linked polystyrene
0.005 0.002 0.00012–0.00025* 0.0004–0.0005†
0.006 0.002 0.00012–0.00066* 0.0005
* Condition A, 10 MHz. † Condition A, 10 GHz.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
62
Chapter Two
TABLE 2.13
Permittivity and Dissipation Factors of FR-4 (Condition D 24/23) Frequency
Dielectric constant
Dissipation factor
100 Hz 1,000 Hz 10,000 Hz 100,000 Hz 1 MHz 10 MHz 100 MHz 1,000 MHz 10,000 MHz
4.80 4.75 4.70 4.65 4.60 4.55 4.50 4.45 4.40
0.009 0.012 0.015 0.018 0.020 0.022 0.024 0.025 0.025
material either by depositing the initial layer in a patterned fashion (screen printing) or by the use of a master of the pattern desired and a photographic sequence of exposing and developing for copying the master to the polymer coating. The choice between these patterning sequences is governed by the feature size desired. Larger features (8 mil and greater) can be very economically formed by screen printing. Feature sizes smaller than 8 mil are formed using a photolithographic process.
Clean Surface
Apply Photoresist
Expose Photoresist
Develop Photoresist Image
Pattern Transfer Image (plating or etching)
Strip Photoresist Process flow chart of photolithography.
Figure 2.14
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
63
2.4.1.1 Photosensitive materials. The photosensitive polymeric systems used in the PCB industry are used either as liquids directly or as dry films of an initial liquid solution. Both types of materials are used widely and are excellent solutions for a variety of processing requirements. In addition, these materials may function in a photographic sense in a positive or negative tone. The difference is illustrated in Fig. 2.15 and arises from the distinct chemical compositions and in the photoinitiated reaction within the film itself. The key factor to the functioning of these materials is that their solubility in the developing solution changes on exposure to light. In the case of the common negative-acting systems, the photoreaction provides a polymer network that is less soluble in the developing solution by promoting cross-linking between one or more of the components in the polymeric matrix. The resulting molecular weight change in the exposed region of the film reduces the material’s solubility, and it is these regions that remain after development of the image. In the positive-acting systems, the chemistry is very often that of the novalac resin-based materials utilized by the semiconductor industry. Upon irradiation, the material becomes more soluble than the original, and it is these exposed regions that are removed in the developer solution. There are many reports of the inherent differences in product yield associated with either positive- or negative-acting material. Positive-acting materials are often considered to provide for a higher-yield process. This could be due to the division of lines and spaces on the phototool; spaces are a greater area than lines. For a positive-acting material, the spaces are clear and these large areas are less sensitive to defect-causing debris. In contrast, for negative phototools, a small size and amount of contaminant will be reproduced as an open in the conductor. It is unfortunate that there are few materials that don’t have some other obvious attribute such as thickness, coating method, etc., which will alter the yield other than their photographic tone. There is a large variety of materials commercially available, but how does one determine which is likely to perform best for a given application? There are several key factors to consider—several technical and many economic, the latter of which are unique to each manufacturing facility. The technical decision sequence is summarized in Fig. 2.16. The foremost consideration is the end use of the pattern; the material must have chemical compatibility with the subsequent pattern transfer steps. The chemical nature of these steps, especially the solution pH, must be distinct from the photoresist’s unique solubility. Only then can the photoresist perform as an accurate mask for pattern transfer. Another key factor is the nature of the substrate itself in terms of topography and surface features; i.e., is the mask required to cover or tent plated through-holes or tooling features, and must it conform to
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
64
Chapter Two
Figure 2.15 Procedures for positive and negative tone photoresists.
existing circuitry? This consideration will dictate whether dry film or liquid material is appropriate and, in some instances, the required tone of the photoresist material. Equally important is the required product feature dimension and allowable variation. This is usually specified in terms of line width and spacing with a given allowable variation on the nominal. Since these product parameters are for the final conductor features, some estimate of the photoresist processing contribution to this value must be established. Each material has its inherent contrast or ability to switch from exposed to unexposed. This, along with the resist thickness, phototool, and light source used for exposure, governs the feature dimensions that can be defined with a given material. For the materials used in the PCB industry, the following rule usually holds: the minimum line width definable in production is usually 0.5 to 1.0 mil greater than the photoresist thickness. New process sequences have demonstrated improvements beyond this traditional barrier.5 Of a more practical nature, the material chosen must have adhesion to the underlying substrate. There are many approaches to promoting adhesion between dissimilar materials, but there must be an inherent compatibility.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.16
65
Selection criteria for photoresist materials.
2.4.1.2 Equipment alternatives. The process steps for obtaining a usable image are all interactive and, therefore, the equipment plays a very large role in the success of the overall process. For each step there are numerous options. The choice between options is governed by the product specifications with respect to layer thickness and feature size and, in some instances, by the chosen photoresist, in addition to the economic factors that are unique to each installation. The alternative equipment for each process step will be described with criteria by which to compare them. Cleanliness considerations. Cleanliness is of concern for the entire photolithography process. This includes yellow room contamination level
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
66
Chapter Two
(cleanliness class), solution filtration, equipment cleanliness class, and product handling. The relative importance of each of these must be established for the product feature dimensions. The sensitivity of the photolithographic sequence to the size and location of contamination can be determined, and then the appropriate level of cleanliness can be instituted and maintained.6–8 In addition, equipment to remove contamination from flat surfaces—either panels or equipment—can be used throughout the processing sequence. These sticky rollers are available as freestanding equipment and as handheld items. Preclean. This step provides the foundation for all the others since only an appropriately cleaned substrate allows for good adhesion between the photoresist and the substrate and for the remainder of the process to be successful.9 All laminates arrive at the imaging area dirty and, depending on the type of contamination, the exact process sequence is chosen. Contamination—epoxy dust—from trimming and processing the laminate itself is removed by mechanical cleaning. The surface copper is either foil or foil with electroless or electroplated copper. The foil is treated with an antitarnishing agent of chromium and zinc, which is removed for reproducible imaging results. Not only are contaminants removed, but also the texture or surface roughness of the copper is altered to promote mechanical adhesion between the base copper and the photoresist. The extent of this texturing is measured by the usual parameters for surface roughness where the height and spacing of the topography is quantified by profilometer measurements (see Fig. 2.17). Chemical cleanliness can be determined in a variety of ways. Wetting is often tested using a water break test or more analytically in terms of contact angle where a low value is desirable. In addition, analytical techniques can be used to evaluate the chemical composition of the surface (Auger and x-ray photoelectron spectroscopy [XPS]) (Table 2.14). Photoresist apply. The numerous choices for applying the photoresist are tied in most instances to the photoresist choice. The discussion here will be divided between liquid and dry film methods. Irrespective of the method chosen, the cleanliness of the operation—both the equipment and the clean room—and the handling of the product are important. It is also advisable to minimize the handling at this stage with the use of automated operation. Specifically, in-line equipment, with the preclean step and automatic loading and unloading, is advised. Expose. In this key step for image formation, the master pattern is aligned to and exposed in the product so that the relief image can be subsequently developed. The elements of the process are the phototool, the registration of the phototool to the panel, and the light source used for exposure. The choices for phototools (film or glass) differ as to sharp-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.17
67
Surface roughness parameters.
ness of the transition from opaque to clear, the pattern’s dimensional stability, and the substrate absorption of the exposing light. The panel is aligned either mechanically with pins holding the phototool with respect to the product or optically with alignment features dictating the movement of the phototool and product. The alignment requirements are interrelated with those achieved at composite lamination and drilling. The registration scheme is contained within the exposure equipment. The light source alternatives include contact printing with either a collimated or uncollimated light source, proximity printing, projection printing, and laser direct imaging.10 The latter three methods separate the phototool from the substrate and are expected to have an increased product yield due to reduced contamination. No phototool is used in laser direct imaging since the laser beam exposes the image based on the design data. TABLE 2.14
Sample Initial Preclean 1 Preclean 2
Copper Surface Chemical Composition as Measured by XPS % Cu
%O
%C
12 6
46 19 10
24 68 70
%N
% Zn
% Cr
16
12
14
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
68
Chapter Two
Develop. In this process step, the solubility difference between the exposed and unexposed portions of the photoresist is realized. Immersion in an appropriate solvent results in a relief image of the master pattern. The process conditions are adjusted to alter the clearing time for dissolving the unexposed or negative materials or exposed or positive ones. The total dwell time is set to approximately double the time to clear, commonly called a 50 percent breakpoint. Additional variables include the solution temperature, agitation, and concentration. The resulting photoresist images should be distinct with vertical sidewalls. Failure to accomplish this is an indication that the previous process step setpoints require adjustment. Images larger than the phototool dimension result from incomplete development, overexposure, or poor contact at expose. If the images are smaller than expected, then the exposure dose is too low or development is too aggressive. Distorted images can be caused by problems with precleaning, application, or exposure. The common equipment for developing is spray conveyorized, either horizontally or vertically. Additives to the developer solution are required in many instances to prevent foaming. The solution is filtered to remove resist particles and either replenished with fresh solution to maintain a consistent dissolved resist value and solution concentration or operated continuously for a certain amount of product and replaced. Waste developer solution is treated (aqueous and semiaqueous) or distilled and reused (solvent). Rinsing is also important to stop the dissolution reaction. In addition, water with a high mineral content often improves the aqueous photoresist resist image and the conductor yield. Tank systems can also be used, especially for materials with a wide process latitude. Often, ultrasonic agitation is used to aid in the dissolution. There are additional steps that improve the resist removal in the line channels and the conductor formation yield. Plasma treatment has been used effectively to improve product yield, especially with respect to shorts in a print-and-etch process. In addition, for some aqueousdevelopable dry films, a heat treatment after exposure improves the space definition, and spaces equal to or smaller than the resist height have been resolved.5 Thus, these process steps ensure that tight resolution requirements can be met. Strip. The photoresist is removed from the substrate after it has functioned in the pattern transfer step. The equipment used for this process step is identical to that used for developing. The removal is accomplished by swelling and dissolving the material. Some materials are removed in sheets or as small particles and, depending on the equipment design, can be accommodated. Often brushes and ultrasonic
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
69
agitation are added to aid in the resist removal. As with developing, filtration is important to keep fresh solution reaching the part and the nozzles of a spray tool clean. For stripper chemistries that oxidize the copper, an antitarnishing agent is often added to either the stripping or rinsing solution. 2.4.1.3 Design for manufacturing. A high-yield conductor formation process can be enhanced by the optimization of several design features. These concern the conductor dimensions and the process used to form them. Specifically, these are the process sequence to be used (etched or plated metal), the division of conductor pitch between line and spacing, and the PTH capture land size and shape. Process sequence: etch vs. plate considerations. For a given product conductor dimension, there is often a question of the appropriate process sequence. Although the capabilities of imaging and the pattern transfer step dictate the overall limitations, the decision depends on the unique capabilities of the manufacturing line to be used. Some general considerations can clarify the true issues for most production situations. The photoresist patterns for plating and etching are very distinct. For etching, a thin photoresist is desirable to maximize the etchants’ attack in the line channel. Thus, the resolution of the photoresist does not limit the process, since very small spaces can be resolved in liquidcoated materials. The challenge for conductor formation resides with the etching. Depending on the metal thickness and the etching equipment, it can be very difficult to remove the copper in tight spaces. Therefore, the key criterion defining the capabilities of the print-andetch process is the minimum spacing cleared as constrained by the final conductor height and the etchant chemistry and equipment. For plated products, the photoresist thickness must be greater than or equal to the final thickness of the conductor wire and it must be possible to clear a photoresist space equal to the final conductor width. These fine spaces are challenging when the conductor height increases. The photoresist resolution is on the order of its thickness, so that for 1-mil-thick plating, it would be difficult to resolve a photoresist space smaller than 1.5 mil, irrespective of the final conductor spacing. Thus, the challenge for plating is to resolve the fine spaces in thicker photoresist materials and then to ensure that the plating solution wets the bottom of the narrow photoresist channels. Thus, in choosing the conductor formation process, the thickness of the conductor and the line width and spacing are the key parameters. A generalized relationship between them is found in Fig. 2.18. It is important that this type of plot is known for the production area before the process sequence is determined.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
70
Chapter Two
2
1.8
1.6
Cu Thickness (mils)
1.4 1.2
1 0.8
0.6 0.4
0.2 0 2
4
5
9
10
Line / Space Pitch (mils)
Figure 2.18
Typical manufacturing line process capability to aid in sequence decisions.
Line and space division for a fixed pitch. It is common for product designs to have a fixed pitch, whether it refers to the I/Os for direct chip or packaging attachment or to the spacing between PTHs. This space is often divided equally between conductors and spacing. As mentioned previously, for either additive or subtractive processing, the photoresist and pattern transfer process yield can be enhanced by avoiding the resolution limitations of each sequence. In subtractive conductor formation, an etch factor is used to obtain straighter sidewalls and improved line width control. If lines and spaces are equally allocated, then the photoresist must resolve a smaller space than a line. This is difficult, except when very thin coatings are used in conjunction with one of the enhancement schemes.5 Thus, it is a higher-yielding process to have larger spaces than lines. For additive processing, the spacing in the photoresist is the limiting factor. After pattern transfer, this will become the line. In this instance, equal lines and spaces are more acceptable, but based on the photoresist concerns, a wider final line than space is preferred. At the same time, it is desirable to increase the spacing for reduced incidence of line shorting, which translates to a wider “line” in the photoresist. The former is usually more important. Therefore, for both process sequences there is preferably balance between line width and spacing. PTH capture pad size and shape for optimum line formation. Just as the conductor line and spacing can be optimized, the PTH capture pad shape and size can be altered to further increase the yield. The absolute
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
71
dimension of the feature is dictated by the placement accuracy of the drilling process and the overall dimensional stability of the product. The feature is sized to ensure that the PTH and conductor are connected. There are varying specifications as to the extent of capture that is required. Depending on the direction and magnitude of the dimensional stability and the drill wander and accuracy, the shape required to capture the PTH can be changed. This would reduce the size of this feature in at least one direction. In consequence, the spacing between the line and pad increases. Since this location is a change to the nominal line-to-line spacing, the narrowing of the channel results in shorting between the features in both print-and-etch and additive processes. In the former case, it is more difficult to clear the space, and in the latter, the narrower resist width is often underplated. Thus, when possible, an elongated pad will benefit the final conductor yield. 2.4.2 Drilling processes
The purpose of drilling printed circuit boards is twofold: (1) to produce an opening through the board that will permit a subsequent process to form an electrical connection between top, bottom, and sometimes intermediate conductor pathways; and (2) to permit through-theboard component mounting with structural integrity and precision of location. The quality of a drilled hole through a printed circuit board is measured by its interface with the following processes: plating, soldering, and forming a high-reliability nondegrading electrical and mechanical connection. It is possible to drill holes meeting these requirements with high productivity, consistency, and yield. The elements of this process are materials, such as laminates, drill entry, and backup, and drills; processes including machine parameters, techniques, and operating personnel; and control evaluation of hole quality, drills, and process machinery. When all these elements are properly developed and implemented, high-quality printed circuit board holes are a natural result. Such holes can be plated directly, eliminating remedial processes of deburring, desmearing, and etchback, and resulting in process simplification, higher yields, and lower costs. The interaction and practice of elements shown in Fig. 2.19 can optimize the drilling process for the fabrication of printed circuit boards. While all of the elements shown are interdependent, it is hole quality and location accuracy that ultimately steer decisions on feeds and speeds, material choices, and productivity.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
72
Chapter Two
Figure 2.19
Essential elements of successful PCB drilling.
2.4.2.1 Drills. Drills for making holes in printed circuit boards are usually made of tungsten carbide. This is due to interrelated needs of cost, wear properties, machinability, and handling properties. No other material has proved to be as suitable. The design of a drill is just as important as the materials used. The design and the wear of the drill affect its drilling temperature, ability to remove chips, tendency to create entry and exit burrs, and smoothness of the hole wall (all directly related to hole quality). Figure 2.20 shows a typical drill bit geometry. The point angle is usually between 90° and 110° for paper-base materials and between 115° and 130° for glass-base materials. By far the most common point angle
Figure 2.20
Typical drill bit geometry.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
73
used in drilling is 130°. The flute or helix angle determines the drill’s ability to remove chips from the hole. Helix angles vary from 20° to 50°. A 20° angle provides fast chip removal with poor cutting efficiency. A high helix angle (50°) creates a smaller material plastic zone but yields slower chip removal, as shown in Fig. 2.21, angle A. A helix angle of 30° is a good compromise between a small plastic zone and quick chip removal. This compromise minimizes drilling temperature. Figure 2.20 also shows an important characteristic of highperformance drills described as a relieved land. Increases in temperature during drilling can also be caused by the amount of drill surface area in direct contact with the hole wall. To minimize this surface area, most manufacturers remove material just behind the margin or cutting area to reduce friction and thus lower the temperature of drilling. Other geometries being equal, the narrower the margin, the cooler the drilling temperature. The length of the margin relieved area also affects the drilling temperature. Figure 2.22 shows the relief area in a (a) partially relieved, (b) fully relieved, and (c) spade-head drill. A drill design with a larger relief area will drill cooler because of the smaller drill surface area in contact with the hole wall. Other factors being equal, the partially relieved design will drill hotter than the fully relieved design and the spade head design will drill cooler than the fully relieved design. The surface finish of the drill is important; that is, the smoother the surface, the cooler the drilling. Surface finishes lower than 4 µin. should be used. The volume of empty space in the drill flutes is another important design consideration. The greater the open volume, the higher the capacity of the drill to remove chips efficiently. Conversely, greater volume (thinner center web) implies a weaker drill that is more prone to breakage. Figure 2.23 shows (a) a standard microdrill and (b) a step design that strengthens the drill without increasing the web thickness by adding a step in the diameter reduction between the drill shank and the fluted area. The added step strengthens the drill bit by
Schematic diagram for the cutting process of drill bit.
Figure 2.21
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
74
Chapter Two
Figure 2.22 Drill bit flute designs. (a) Partially relieved. (b) Fully relieved. (c) Spade-head.
reducing the abruptness of the transition between the flute and the shank of the drill bit. In general, the best drill designs are those that drill with the lowest drill temperature. Drills that drill cooler have a good surface finish, thin webs, no geometrical defects or chips, sharp cutting edges, and durable carbide. In addition, the best operating parameters for drills are those that also minimize drill temperatures. Finally, as drills wear, they drill hotter and hole quality decreases. Run length must be carefully determined. It should not be assumed that all manufactured drills are of equal quality. Differences in design, manufacturing processes, surface finish, raw materials, and consistency vary widely and should be evaluated prior to the purchase of production quantities of drills. 2.4.2.2 Laminates. All laminates are manufactured to specifications that take into account electrical and physical properties. Ease of drilling ordinarily is not considered by laminate engineers. It is left up to the printed circuit board fabricator to develop the correct parameters to drill laminates for the best hole quality. The various types of laminates are formed from several resins and supporting materials. These vary from common to exotic types that differ in the ease with which they may be drilled. From easiest to most difficult to drill, some commonly available laminates are G-10 epoxy-glass, FR-4 epoxy-glass, multifunctional epoxy, polyimide-glass, phenolic-paper, Teflon-glass, polyimide-quartz, and exotics.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
Figure 2.23
75
Geometry of microdrill bits. (a) Standard design. (b) Step
design.
Where cloth is used, the weave and fiber thickness affect drill wander. The finer the fiber, the less drill wander. In addition, laminate is produced with various thicknesses of copper, either in double-sided laminates or in multilayers. The ratio of the copper thickness to total thickness of the laminate changes the optimum drilling parameters so that feeds and speeds should be adjusted based on the ratio of copper to substrate. Dimensional stability, warping, bow, and twist specifica-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
76
Chapter Two
tions are important to the drilling operations. For example, laminates that are not flat drill with high burrs. The thickness of the laminate to be drilled is controlled by the smallest drill diameter to be used. The controlling factor is 10 times the drill diameter. For example, the maximum material thickness for a 0.020-in.diameter drill is 0.200 in. As drill depth increases, the drill’s deviation from true center increases. For minimum-sized drills, the deviation increases by 0.001 in. for each 0.0625 in. of laminate thickness. For example, a 0.020-in.-diameter drill drilling through 0.200-in. laminate provides deviations of 0.005 in. If this is unacceptable, laminate thickness must be reduced. Good multilayers and double-sided laminates should not require prebaking before drilling to fully cure the laminate. Uncured laminate is unacceptable from the supplier. Prebaking is often practiced to stress-relieve the laminate. Edges of laminate panels for drilling should be free of burrs so that stacking can occur with good interlaminate contact. To produce quality holes for each series or type of laminate, the following generalities can be stated: ■
The higher the Tg of the laminate, the better.
■
The laminate should be flat, uniform in thickness, and smooth, and it should exhibit high copper peel strength.
■
Prebaking the laminate before drilling helps dimensional stability but does not “correct” uncured resin.
■
The storage of laminate under controlled conditions of temperature and humidity is necessary. These conditions should be the same as the ambient conditions surrounding the drilling machine.
■
The more glass cloth layers and the higher the glass-to-resin ratio, the more drill wear is obtained per hole drilled.
■
The thicker the glass cloth diameter, the greater the drill wander.
■
Laminates that are not flat will cause interlaminate entry and exit burring.
■
The more abrasive the supporting fibers (quartz, for example), the greater the drill wear and the shorter the drilling run per drill.
■
Harder and thicker copper shortens the life of the drill.
Laminate panels are normally stacked three high between entry and backup materials for 0.062-in.-thick double-sided laminates and one or two high for multilayers. They are placed in a pinning machine that drills a minimum of two holes and inserts tooling pins to hold the stack firmly.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
77
Foreign materials and burrs on the laminate must be removed. This is true for entry and backup materials as well. The stack must be tight. Loose pinning causes burrs and poor registration. Poor pin alignment can cause bowed stacks. Pins and bushings should be checked for wear, and drilling machine operators should be instructed on the importance of cleanliness when handling laminates and entry and backup materials. 2.4.2.3 Drilling machines. Drilling machine types vary over a wide range, from single-spindle, manually operated, bottom-drilling types, using templates for locating holes, to multiple-drill-station, computer numerically controlled (CNC), automatic machines that accept stacks of laminate, eject laminate, and change tools automatically. Machines are designed to accept laminate panels of various sizes, up to 24 × 24 in. Costs range from $10,000 at the low end to $500,000 for the largest and most automated machines. The type of machine needed depends on production capacity and the type of process design. Whatever the type, it is important to prepare and design the machine’s environment. Machines should be located in temperature- and humiditycontrolled, dust-free environments. Floors should be adequately designed to carry the machine weight. Machines should be isolated from any external vibrations. Isolated electrical power and grounding are necessary. Rigorous and well-planned maintenance programs are important. The items in the following list are most important, but the list is not inclusive.
1. The actual revolutions per minute and feed rate of the machine should be determined by an independent method. Do not rely on the machine readout. 2. Vacuum systems should be maintained at high flow rates and full efficiency. It is better to overdesign this function. Filters should be replaced regularly. 3. Spindle cooling systems, coolant, and heat exhangers should be checked and kept clean so that they work efficiently. 4. Spindles and collets should be kept clean at all times, using noncorrosive cleaners that keep thin protective films on the metallic parts. 5. Spindle runout should be kept to less than 0.0005 in. for heart of the range drilling and to less than 0.0002 in. for small hole drilling. 6. Drill bars, springs, and air-pressure seals should be carefully checked and maintained. 7. Pressure foot pressures should remain as high as the laminate will allow. 8. The z-axis alignment should be checked often.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
78
Chapter Two
Machine manufacturers’ instructions regarding warmup before use should be followed carefully. Machines should be kept scrupulously clean. Dirt, chips, and debris left on machine tables should be removed with a vacuum cleaner. Never blow surfaces with compressed air to remove dirt. There are two aspects to drill wander: precision and accuracy. Only accuracy is affected by machine performance. The machine accuracy can be checked by drilling a square matrix of holes. The lines of holes can be defined in the x and y directions by comparing the mean lines to reference holes via regression analysis. These best-fit lines are compared with the desired lines the machine was instructed to place. From the slopes, the orthogonality of the machine can also be determined. Precision of drilling is dependent on many factors. One of these is spindle runout. The less the spindle runout, the greater the precision of drilling. With good spindles and a well-maintained machine, precision and accuracy are about equal for 0.0135-in.-diameter drills. These calculations are based on drilling 0.100 in. of laminate. Precision is also affected by chip load, roughness of laminate surface, entry material roughness, entry material construction, drill bit diameter, glass weave, glass thickness, drill design, and drill concentricity. 2.4.2.4 Accuracy and precision. It is important to understand how to produce not only high hole quality but also accurate, precisely drilled holes. Accuracy can be defined as how well the hole location agrees with the correct or target value. Precision is defined as how reproducible the hole location is. Accuracy problems are usually due to drilling machine problems. Machine problems are due to mechanical wear, loss of computer data, and electromechanical error. Precision problems are due to poor entry material, laminate thicknesses that are too great for the drill diameter, excessive chip loads, drill resonance, and excessive spindle runout. 2.4.3 Plating processes
A major part of manufacturing printed circuit boards involves wet process chemistry. The plating aspects of wet chemistry include deposition of metals by electroless (metallization) and electrolytic (electroplating) processes. Topics to be described here are electroless copper, electroplating of copper and resist metals, nickel and gold for edge connector (tips), tin-lead plating, and alternative coatings. Specific operating conditions, process controls, and problems in each area will be reviewed in this section. (See printed circuit plating flowchart in Fig. 2.24.) Two driving forces have had major influence on plating practices: the precise technical requirements of electronic products and the demands
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
79
Plating flowchart for printed circuit board manufacturing.
Figure 2.24
of environmental and safety compliance. Recent technical achievements in plating are evident in the capability to produce complex, highresolution multilayer boards. These boards show narrow lines (3 to 6 mil), small holes (12 mil), surface-mount density, and high reliability. In plating, such precision has been made possible by the use of improved automatic, computer-controlled plating machines, instrumental techniques for analysis of organic and metallic additives, and the availability of controllable chemical processes. Mil-spec-quality boards are produced when the procedures given here are closely followed. 2.4.3.1 Electroless copper plating.11–15 This series of chemical steps (after smear removal) is used to make panel side-to-side and innerlayer connections by metallizing with copper. The process steps needed include racking, cleaning, copper microetching, hole and surface catalyzing with palladium, and electroless copper. Typical steps are as follows:
1. Cleaner-conditioner. Alkaline cleaning is used to remove soils and condition holes.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
80
Chapter Two
2. Microetch. This slow acid etching is used for removal of copper surface pretreatments, oxidation, and presentation of uniformly active copper. Persulfates and sulfuric acid–hydrogen peroxide solutions are commonly used. 3. Sulfuric acid. Used for removal of persulfate residues. 4. Predip. Used to maintain balance of the next step. 5. Catalyst (activator). Neutral or acid solutions of palladium and tin are used to deposit a thin layer of surface-active palladium in the holes and on the surface. 6. Accelerator (postactivator). Used for the removal of colloidal tin on board surfaces and holes. 7. Electroless copper. Alkaline-chelated copper reducing solution that deposits thin copper in the holes (20 to 100 µin.) and on surfaces. 8. Antitarnish. A neutral solution that prevents oxidation of active copper surfaces by forming a copper conversion coating. Selection from several types available depends on the type of image transfer desired. Operation and control of three bath types and the function of constituents are given in Tables 2.15 and 2.16. The following outline presents the typical steps in an electroless copper process: 1. Rack 2. Clean and condition 3. Water rinse 4. Surface copper etch (microtech) TABLE 2.15
Operation and Control of Electroless Cu Processes Low deposition
Medium deposition
Heavy deposition
Copper HCHO NaOH Temperature Air agitation Filtration Tank design
3 g/l 6–9 g/l 6–9 g/l 65–85°F Mild Periodic Static
Heater Panel loading Replenish mode
Teflon 0.25–1.5 ft2/gal Manual
2.0 g/l 3.3 g/l 8 g/l 115 ⫾ 5°F Moderate Continuous Overflow, separate sump Teflon 0.1–2.0 ft2/gal Automatic
Idle time, control Deposition time Thickness
70–85% 20 min 20 µin.
2.8 g/l 3.5 g/l 10–11 g/l 115 ⫾ 5°F Mild/moderate Continuous Overflow, separate sump Teflon 0.1–2.0 ft2/gal Manual or continuous Turn off heat 20 min 40–60 µin.
Turn off heat 20–30 min 60–100 µin.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
TABLE 2.16
81
Function of Constituents for Electroless Cu Plating Constituent
Copper salt Reducing agent Complexer pH controller Additives
CuSO4 ⋅ 5 H2O HCHO EDTA, tartrates, Rochelle salts NaOH NaCN, metals, S, N, CN organics
Function Supplies copper Cu+2 + 2e → Cu0 Holds Cu+2 in solution at high pH; controls rate Controls pH (rate) 11.5–12.5 optimum for HCHO reduction Stabilize, brighten, speed rate, strengthen
5. Water rinse 6. Sulfuric acid (optional) 7. Water rinse 8. Preactivator 9. Activator (catalyst) 10. Water rinse 11. Postactivator (accelerator) 12. Water rinse 13. Electroless copper 14. Rinse 15. Sulfuric acid or antitarnish 16. Rinse 17. Scrub (optional) 18. Rinse 19. Copper flash plate (optional) 20. Dry 21. Release to image transfer 2.4.3.2 Copper electroplating. Because of its high electrical conductivity, strength, ductility, and low cost, copper is the most commonly used metal for the structure of a printed circuit board. In addition, copper is readily plated from simple solutions and is easily etched. MIL-STD275 states that electrode-posited copper shall be in accordance with MIL-C-104550, and shall have a minimum purity of 99.5 percent as determined by ASTM E 53. The minimum thickness shall be 0.001 in. (1 mil). Requirements for good soldering also indicate the need for 1 mil of copper and smooth holes.30 Copper plating is generally regarded as the slow step in manufacturing PCBs. New methods that cut plating
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
82
Chapter Two
times by as much as 50 percent include high-speed additives, pulse plating, and rapid solution-impingement machines.16–24 Key factors for uniform plating. To have day-to-day control and to achieve ductile, strong deposits and uniform copper thickness, the following controls are required:25–27
1. Maintain equipment following best practices, such as uniform air agitation in the tank, equal anode-cathode distances, rectifier connection on both ends of tank, and low resistance between rack and cathode bar. 2. Maintain narrow range control of all chemical constituents, including organic additives and contaminants. 3. Conduct batch carbon treatment regularly. 4. Control temperature at 70°F to 85°F. 5. Eliminate contaminants in tank from preplate cleaners, microetchants, and impure chemicals. 6. Plate at one-eighth to one-half of the conventional cathode current density when using thick boards (0.100 in.) with small holes (0.015 in.) and fine lines (6 to 8 mil). Acid copper sulfate. The preferred industrial process uses an acid copper sulfate solution containing copper sulfate, sulfuric acid, chloride ion, and organic additives. Using the proper additives, the resultant copper is fine-grained with tensile strengths of 50,000 lb/in2 (345 MPa), a minimum of 10 percent elongation, and a surface-to-hole thickness ratio of 1.2. (See Table 2.17.) Copper pyrophosphate. Once the standard of the industry, pyrocopper has been almost entirely replaced by acid copper, except in military and special applications. Pyrocopper continues to be used because of its resistance to cracking, high throwing power, and purity of deposits. The use of organic additives with pyrocopper is optional,28–30 but it is preferred because such additives provide wider tolerance of cracking control and improve deposit quality.31–34 The additive PY-61H, identified as dimercaptothiadiazole, is effectively controlled in production by CVS. (See Table 2.18.)
2.4.3.3 Solder (Sn-Pb) electroplating. Solder plate (Sn60-Pb40) is widely used as a finish plate on printed circuit boards. This process features excellent etch resistance to alkaline ammonia, good solderability after storage, and good corrosion resistance. Tin-lead plating is used for several types of boards, including tin-lead/copper, tin-lead/tin-nickel/copper, solder mask on bare copper (SMOBC), and surface-mount (SM). Fusing
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
TABLE 2.17
83
Operation and Control of Acid Cu Sulfate Conventional
Operating variables Copper Copper sulfate Sulfuric acid Chloride Additives Temperature Cathode current density Anodes† Type Composition Bags Hooks Length Anode current density Properties Composition Elongation Tensile strength
2–3 oz/gal 8–12 oz/gal 22–28 oz/gal 40–80 ppm As required 70–85°F 20–40 A/ft2*
High-speed 3–4.5 oz/gal 12–18 oz/gal 24–36 oz/gal 40–80 ppm As required 75–100°F 40–150 A/ft2
Bars or baskets Phosphorized 0.04–0.06% P Closed-napped polypropylene Titanium or Monel Rack length minus 2 in. 10–20 A/ft2 conventional; 25–50 A/ft2 high speed 99.8% (99.5% min, ASTM E 53) 10–25% (6% min, ASTM E8 or E 345) 40–50 kpsi (36 kpsi min, ASTM E 8 or E 345)
* A/ft2 refers to amperes per square foot and is sometimes expressed as ASF. † Operating anodes should have a thin, brown or black, easily removed film.
TABLE 2.18
Operation and Control of Cu Pyrophosphate
Operating conditions pH Copper Pyrophosphate Orthophosphate Ammonia (NH3) Ratio (pyro/Cu) Temperature Cathode current density Aqua ammonia PY 61-H* Anodes† Type Composition Bags Current density Hooks Length
8.1–8.5 copper 2.7–3.5 oz/gal 19.4–26.3 oz/gal 8 oz/gal max 0.2–0.3 oz/gal 7.5–8.0/L 115–125°F 20–35 A/ft2 As needed; about 1–2 qt/day 0.25–0.75 ml/(Ah) Control with CVS Bars or baskets OFHC copper Optional, none required 20–30 A/ft2 Titanium Rack length minus 2 in
* Product of M&T Chemicals, Rahway, N.J. † Operating anodes should have a thin golden or light tan film.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
84
Chapter Two
is required on all tin-lead-plated surfaces. Thickness minimums are not specified. The preferred composition contains a minimum of 55 percent and a maximum of 70 percent tin. This alloy is near the tin-lead eutectic, which fuses at a temperature lower than the melting point of either tin or lead, and thus makes it easy to reflow (fuse) and solder. (The composition of the eutectic is 63 percent tin, 37 percent lead with a melting point of 361°F.) Fusing processes include infrared (IR), hot oil, vapor phase, and hot-air leveling for SMOBC. Plating solutions currently available include the widely used high-concentration fluoboric acidpeptone system, as well as low-fluoboric, nonpeptone, and a nonfluoboric organic aryl sulfonic acid process. These processes are formulated to have high throwing power and give uniform alloy composition.35 The sulfonic acid process has the advantage of using ball-shaped lead-tin anodes but is difficult to operate. Table 2.19 gives details of operation and control of two high-throw tin-lead (solder) baths. 2.4.3.4 Tin electroplating. Tin is used extensively for plating electronic components and PCBs due to its solderability, corrosion resistance, and metal etch-resist properties. The current MIL-STD-275 does not include tin plating, although earlier versions stated a required thickness of 0.0003 in. Specifications covering tin plating are MIL-T-10727 and MILP-38510, which say that tin must be fused on component leads. Acid tin sulfate is the most widely used system. Among the many processes available, some produce bright deposits for appearance and TABLE 2.19
Operation and Control of Sn-Pb Fluoborate High HBF4 /peptone
Lead Stannous tin (Sn+2) Free fluoboric acid Boric acid Additive Temperature Cathode current density Agitation Anodes Type Composition Purity Bags Hooks Length Current density
Low HBF4 /proprietary
1.07–1.88 oz/gal 1.61–2.68 oz/gal 47–67 oz/gal Hang bag in tank Use as needed by Hull cell and Ah usage 60–80°F 15–18 A/ft2
1.4–2.0 oz/gal 2.8–4.0 oz/gal 15–25 oz/gal Same
Solution circulation
Mechanical and solution circulation
70–85°F 10–30 A/ft2
Bar Sn60-Pb40 Federal Specification QQ-S-571 Polypro Monel Rack length minus 2 in. 10–20 A/ft2
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
85
corrosion resistance; others give matte deposits that can be fused as well as soldered after long-term heating. Tin sulfate baths are somewhat difficult to control, especially after prolonged use.36 Operation and control are given in Table 2.20. Nickel electroplating. Nickel plating is used as an undercoat for precious and nonprecious metals. For surfaces such as contacts or tips that normally receive heavy wear, the use of nickel under a gold or rhodium plate will greatly increase wear resistance. When used as a barrier layer, nickel is effective in preventing diffusion between copper and other plated metals. Nickel-gold combinations are frequently used as metal etch resists. Nickel alone will function as an etch resist against the ammoniacal etchants.37 MIL-STD-275 calls for a low-stress nickel with a minimum thickness of 0.0002 in. Low-stress nickel deposits are generally obtained using nickel sulfamate baths in conjunction with wetting (antipit) agents. Additives are also used to reduce stress and to improve surface appearance. Nickel sulfamate is commonly used both as undercoat for throughhole plating and on tips. Conditions given in Table 2.21 are applicable for through-hole and full-board plating. Nickel sulfate is typically plated with an automatic edge connector (tip) plating machine. Table 2.22 gives the operating conditions that apply to these systems. Nickel anodes are preferred in tip machines because the pH and the metal content remain stable. The pH will decrease rapidly when insoluble anodes are used. The pH should be maintained at 1.5 or higher with additions of nickel carbonate. Stress values are higher than in sulfamate baths with values of about 20 kpsi.
2.4.3.5
TABLE 2.20
Operation and Control of Acid Sn Sulfate
Operating conditions Tin Sulfuric acid Carrier, additives Temperature Cathode current density Current efficiency Solution color Plating rate Anodes Type Composition Bags Length Hooks Current density
2 oz/gal 10–12% by volume Replenish by Ah usage and spectrophotometry 55–65°F preferred 65–85°F hazy 20–35 A/ft2 100% Milky, white 0.3 mil @ 25 A/ft2 for 10 min Bars Pure tin Polypropylene Rack length minus 2 in. Monel or titanium 5–20 A/ft2
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
86
Chapter Two
TABLE 2.21
Operation and Control of Ni Sulfamate
Operating conditions pH Nickel As nickel sulfamate Nickel chloride Boric acid Additives Antipit Temperature Cathode current density Anodes Type Composition Purity Hooks, baskets Bags Length
3.5–4.5 (3.8) 10–12 oz/gal 43 oz/gal 4 oz/gal 4–6 oz/gal As required As required 130 ⫾ 5°F 20–40 ASF Bars or chunks Nickel Rolled depolarized, cast, or electrolytic; SD chips in titanium basket Titanium Polypro, Dynel, or cotton Rack length minus 2 in.
Early printed circuit board technology used gold extensively. In addition to being an excellent resist for etching, gold has good electrical conductivity, tarnish resistance, and solderability after storage. Gold can produce contact surfaces with low electrical resistance. Despite its continued advantages, the high cost of gold has restricted its major application to edge connectors (tips) and selected areas, with occasional plating on pads, holes, and traces (body gold). Both hard alloy and soft, pure gold are currently used. Plating solutions are acid (pH 3.5 to 5.0) and neutral (pH 6 to 8.5). Automatic plating machines for edge connectors and manual lines are in use. 2.4.3.6
Gold electroplating.38
Acid hard gold. To a large extent, acid golds are used for compliance to MIL-STD-275, which states that gold shall be in accordance with MILG-45204, Type II, Class 1. The minimum thickness shall be 0.000050 TABLE 2.22
Operation and Control of Ni Sulfate
Operating conditions pH Nickel Nickel chloride Boric acid Stress reducer Antipit Temperature Cathode current density Current efficiency
1.5–4.5 15–17 oz/gal 2–4 oz/gal (with soluble anodes) 3–4 oz/gal As required As required 130 ⫾ 5°F 100–600 A/ft2 65%
Anodes Composition
Nickel or platinized titanium
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
87
in. (50 µin.); the maximum shall be 0.000100 in. in areas that are to be soldered. A low-stress nickel shall be used between gold overplating and copper. Nonmilitary applications require 25 to 50 µin. Type II hard gold is not suited for wire bonding. These systems use potassium gold cyanide in an organic acid electrolyte. Deposit hardness and wear resistance are made possible by adding complexes of cobalt, nickel, or iron to the bath makeup. Automatic plating machines are being used increasingly because of the enhanced thickness (distribution) control, efficient gold usage, productivity, and quality. A comparison of automatic versus manual plating methods for edge connectors is given in Table 2.23. Pure 24-karat gold. High-purity 99.99 percent gold processes are used for boards designed for semiconductor chip (die) attachment, wire bonding, and plating solder (leaded) glass devices due to their solderability and weldability. These qualities comply with Types I and III of MIL-G-45204. The processes are neutral (pH 6 to 8.5) or acid (pH 3 to 6). Pulse plating is frequently used. Table 2.24 gives typical conditions for a neutral bath. Alkaline, noncyanide gold. Various processes for alloy and pure gold deposits are available. Solutions are based on sulfite-gold complexes
TABLE 2.23
Operation and Control of Acid Au-Co Alloy Manual
Gold content, troy oz/gal pH Cobalt content Temperature Solution density Replenishment per troy oz gold Current efficiency Agitation Anode-to-cathode distance Anodes, composition Cathode current density Thickness Deposition rate for 40 µin. Deposition composition Hardness
Automatic
0.9–1.1 4.2–4.6 800–1000 ppm 90–110°F 8–15 Be 8 Ah 50% 5 gal/min 2–3 in. Platinized titanium 1–10 A/ft2 40 ⫾ 10 µin. 3–6 min Au99.8-Co0.2 150 Knoop
1–3 4.5–5.0 800–1200 ppm 100–125°F 12–18 Be 6.5 Ah 60% 50 gal/min 1 ⁄4 in. Platinized titanium 50–100 A/ft2 40 ⫾ 2 µin. 0.3–0.6 min Au99.8-Co0.2 150 Knoop
Gold solution contaminants Metal Lead Silver Chromium Copper
Maximum ppm
Metal
Maximum ppm
10 5 5 50
Iron Tin Nickel
100 300 300–3000
Organics: tape residues, mold growth, and cyanide breakdowns.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
88
Chapter Two
TABLE 2.24
Operation and Control of Neutral Pure Au
Gold content pH Temperature Agitation Solution density Replenishment Current efficiency Cathode current density Deposition rate for 100 µin., 5 A/ft2 Deposit composition Hardness
0.9–1.5 troy oz/gal 6.0–7.0 150°F Vigorous 12–15 Be 4 Ah/troy oz 90–95% 1–10 A/ft2 8 min Au99.99 60–90 Knoop
and arsenic additives and operate at a pH of 8.5 to 10.0. A decision to use this process is based primarily on the need for uniformity (leveling), hardness (180 Knoop), purity, reflectivity, and ductility. PCB use is limited to body plating, since the wear characteristics of sulfite-gold are not suitable for edge connector applications. The microelectronics industry uses these processes for reasons of safety and gold purity. Semiconductor chip attachment, wire bonding, and gold plating on semiconductors are possible applications and are enhanced by using pulse plating without metallic additives. 2.4.3.7 Silver electroplating. Silver is not widely used in the PC industry, although it finds applications in optical devices and switch contacts. Thicknesses of 0.0001 to 0.0002 in. (0.1 to 0.2 mil) in conjunction with a thin overlay of precious metal are specified. Silver plating should not be used when boards are to meet military specification. The reason for this is that, under certain conditions of electrical potential and humidity, silver will migrate along the surface of the deposit and through the body of insulation to produce low-resistance leakage paths. Tarnishing of silver-gold in moist sulfide atmospheres also produces electrical problems on contact surfaces due to diffusion of the silver to the surface. Another reason for the lack of acceptance of silver is that silver is plated from an alkaline cyanide bath, which is highly toxic. Bright plating solutions produce deposits with improved tarnish and corrosion resistance, relative freedom from porosity, and greater hardness. Plating troubles are usually related to black anodes and are due chiefly to solution imbalance, impurities in anodes, or solution roughness and pitting. Most metals to be plated, particularly the less noble metals, require a silver strike prior to silver plating to ensure deposit adhesion. 2.4.3.8 Immersion and electroless plating. Interest in these methods has increased due to their ability to produce coplanar (flat and even pad-to-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
89
pad) surfaces required for fine-pitch, surface-mount devices (SMDs). In effect, these systems offer alternatives to hot-air solder leveling and tinlead alloy plate fusing. These processes are nonelectrolytic. Immersion tin. Immersion tin remains in widespread use to clean boards after etching, to cover copper trace edges with tin, and to act as a soldering aid. Self-limiting by nature, immersion tin processes work by displacement of the copper substrate. Deposits are thin—about 30 µin.—and must be processed immediately for effective results. Aging and thermal excursions cause the growth of the copper-tin intermetallics, which degrades solderability. In addition, tin readily forms a thick oxide when exposed to high temperatures and humidity. Electroless nickel. Electroless nickel (EN) followed by immersion or electroless gold also provides coplanar pad surfaces for SMDs. Electroless nickel is an autocatalytic process that utilizes a reducing agent such as hypophosphite or borohydride. Hypophosphite is the preferred choice for printed circuits. Deposition rate from a bath at pH 4.4 to 5.2 is 1⁄2 to 1 mil/h. The deposit contains 9 to 13 percent phosphorus. EN provides wear resistance, hardness, and excellent uniformity. Thicknesses of 50 to 250 µin. are specified when EN is used as a diffusion barrier between gold and copper. Immersion gold. Immersion gold systems deposit a maximum of 4 to 12 µin. of gold over nickel. Additional gold thickness must be applied by an electroless gold system.
Processes are reported that are capable of depositing 0.5 to 4 mil gold on immersion gold and gold-isolated circuitry by true electroless (autocatalytic) means. These systems contain organic amine boranes and borohydride reducing agents and cyanides and operate at a high pH and temperature. Deposition rate is 80 µin./h. Deposits meet the requirements of MIL-G-45204, Type III, Grade A with 99.9 percent purity and hardnesses of 90 KHN. They are suitable for edge connectors, semiconductor wire bonding, and die attachment. Electroless gold.39
Organic solderability preservatives (OSPs). The OSP processes (also known as prefluxes) are applied to bare copper surfaces after solder mask. Generally, these flat surfaces provide reliable solderability after thermal excursions such as adhesive curing, solder past reflow, and wave soldering, and provided they are adequately protected from oxidation. The OSP must be thermally stable and provide corrosion protection. Options for OSP systems include chemistry based on substituted azoles and rosin/resin bases. The coatings can generally be applied in immersion, spray, or flood mode. The coatings must bind to copper, preventing humidity and high temperatures from degrading solderabil-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
90
Chapter Two
ity, and must be compatible with no-clean assembly fluxes. Proper surface preparation of the boards is required for OSP coatings to be effective. An alternative to this process is the use of benzotrizole. However, this is an extremely thin coating that gives very limited protection against oxidation and moisture. Improved protection can be achieved by following the benzotrizole step with posttreatment of a preflux. The preflux will prevent moisture penetration.40 Both solvent-based and water-based prefluxes are available. The following points should be considered when deciding on alternative coatings previously described. 1. Ease of assembly. Fine-pitch technology may require immersion tin or other electroless plating systems. Mixed-technology boards may be better suited for OSP coatings. 2. Rework and handling. OSP coatings are the easiest to rework but are the most fragile compared to metallic systems. OSPs can be removed with organic solvents or with 5 percent hydrochloric acid if the OSP is a water-based structure. 3. Shelf life. The shelf life of immersion, electroless-plated, and OSP coatings is not as long as that of leveled or fused solder surfaces. Storage time should be kept to a minimum for alternative coatings. 2.4.4 Etching processes
One of the major steps in the chemical processing of subtractive printed boards is etching (removal of copper) to achieve the desired circuit patterns. Etching is also used for surface preparation with minimal metal removal (microetching) during inner-layer oxide coating and electroless or electrolytic plating. Technical, economic, and environmental needs for practical process control have brought about major improvements in etching techniques. Batch-type operations, with their variable etching rates and long downtimes, have been replaced with continuous, constant-etch-rate processes. In addition, the need for continuous processing has led to extensive automation along with complete, integrated systems. The most common etching systems are based on alkaline ammonia, hydrogen peroxide–sulfuric acid, and cupric chloride. Other systems include persulfates, ferric chloride, and chromic-sulfuric acids. Process steps include resist stripping, precleaning, etching, neutralizing, water rinsing, and drying. This chapter describes the technology for etching high-quality, fine-line (0.004 to 0.006 in.) circuits in high volume at a lower cost, as well as closed-loop continuous processing, constant etch rates, control at high dissolved copper capacities, regenerationrecovery, less pollution, and increased safety. Problems of waste dis-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
91
posal and pollution control have been minimized by adapting these principles. Typical procedures are given for etching organic (i.e., dry film) and metal-resist boards, and for inner layers. Strippers and procedures for resist removal are described based on resist selection, cost, and pollution problems. The properties of available etchants are also described in terms of finish plate compatibility, control methods, ease of control, and equipment maintenance. Other considerations include chemical and etchant effects on dielectric laminates, etching of thin-clad copper and semiadditive boards, SMOBC, equipment selection techniques, production capabilities, quality attained, and facilities. 2.4.4.1 General etching considerations and procedures. Good etching results depend on proper image transfer in both organic inner layer print-and-etch and plated-metal etch resists. Etch personnel must be familiar with screened, photosensitive, and plated resists commonly used. The etching of printed boards must begin with suitable cleaning, inspection, and pre-etch steps to ensure acceptable products. Plated boards also require careful and complete resist removal. The steps after etching are important because they are necessary to remove surface contamination and yield sound surfaces. This discussion considers the various types of resists and outlines typical procedures used to etch printed boards using organic and plated resist patterns. Screened resists. Screen printing is a common method for producing standard copper-printed circuitry on metal-clad dielectric and other substrates. The etch resist material is printed with a positive pattern (circuitry only) for copper etch-only boards or with a negative image (field only) when plated through-holes and metal resist are present. The type of resist material used must meet the requirements for proper image transfer demanded by the printer. From the metal etcher’s point of view, the material needs to provide good adhesion and etch solution resistance; be free of pinholes, oil, or resin bleed-out; and be readily removable without damage to substrate or circuitry. Typical problems are excessive undercutting, slivers, unetched areas, and inner-layer shorts in multilayer boards. In addition, conductor line lifting may occur when the copper-to-laminate peel strength is below specification. Hole plugging. Plugged-hole, copper-only boards use alkaline-soluble screen resists in a unique manner. The technique, called hole plugging, makes the SMOBC board possible. UV-cured screen resists. Ultraviolet-cured solventless systems are available for print-and-etch and plating applications. These products are resistant to commonly used acidic plating and etching solutions. Stripping must be evaluated carefully.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
92
Chapter Two
Photoresists. Dry film and liquid photoresist materials are capable of yielding fine-line (0.004 to 0.006 in.) circuits needed for production of surface-mount circuit boards. Like screened resists, photosensitive resists can be used to print either negative or positive patterns on the metal-clad laminate. Although dry film and liquid materials differ in both physical and chemical properties, they will be considered together for our purpose. In general, both positive- and negative-acting resists offer better protection in acidic rather than alkaline solutions; however, negative-acting types are more tolerant of alkaline solutions. Negative resists, once exposed and developed, are no longer light-sensitive and can be processed and stored in normal white light. The positive resists remain light-sensitive even after developing and must therefore be protected from white light. Liquid photoresists, although less durable, are capable of finer line definition and resolution. Positive-acting resists are subject to the same problems as are negative-acting resists, although they are easier to remove cleanly, after exposure, from areas to be etched or plated. Plated etch resists. At present, the most extensive use of metal-plated resists is found in the production of double-sided and multilayer plated through-hole circuit boards. The most commonly used resists are solder plate (Sn60-Pb40), tin, nickel, tin-nickel, and gold. Silver is used to some extent for light-emitting and liquid crystal applications. Etching of the metal-resist-plated boards begins with removal of the resist using commercial solvents and strippers. Gold, solder, and tin resists must be handled carefully because they scratch very easily. Tinnickel alloy and nickel plate, however, are very hard and resistant to abrasion. The procedure after etching includes thorough water rinsing and acid neutralizing to ensure removal of etchant residues on the board surface and under the traces. Alkaline etchants are followed by treatment with proprietary ammonium chloride acidic solutions, ferric and cupric chloride with solutions of hydrochloric or oxalic acid, and ammonium persulfate with sulfuric acid. Alkaline cleaning is used for tinlead boards etched in chromic-sulfuric acid. Etchant residues not removed before drying or reflow result in lowered electrical resistance of the dielectric substrate and in poor electrical contact and soldering on the conductive surfaces.
Resist removal. The method used for resist stripping is important when a resist is selected. The effect on board materials, cost and production requirements, and compliance with safety and pollution standards must be taken into account. Both aqueous and solvent stripping systems are widely used.
2.4.4.2
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
93
Screen resist removal. Alkali-soluble resist inks are generally preferred. Stripping in the case of thermal and UV-curable resists is accomplished in 2 percent sodium hydroxide or in proprietary solutions. The resist is loosened and rinsed off with a water spray. Adequate safety precautions must be taken, since caustics are harmful. Conveyorized resist-stripping and etching machines use highpressure pumping systems that spray hot alkaline solutions on both sides of the boards. Single-sided boards and certain laminate materials such as the polyimides may be attached by alkaline strippers. Measling, staining, or other degradation is noted when strippers attack epoxy or other substrates. Screened vinyl-based resists are removed by a dissolving action in solutions of chlorinated, petroleum, or glycol ether solvents. Methylene chloride and toluene are used extensively in cold stripper formulations.41 Commercial cold strippers are classified according to their pH in a 10 percent stripper-water mixture. The most common strippers are acidic formulations that contain copper brighteners and swelling, dissolution, and water-rinsing agents. The usual procedure for static tank stripping involves soaking the coated boards in at least two tanks of stripper. Excessive time in strippers is to be avoided because of attack on the “butter” (top epoxy) coat, especially on print-and-etch or singlesided boards. Water is a contaminant in most cold strippers. Solvent stripping machines are commercially available. High-volume users save costs by using conveyorized systems equipped with reclamation and pollution-control facilities. Distillable cold strippers generally contain methylene chloride or trichloroethylene (TCE). Some heating may be used, but only in closed systems because of health and fire hazards. In all cases, proper safety, ventilation, pollution control, and certified waste disposal must be provided. Methylene chloride, toluene, and TCE are priority pollutants (TTO) regulated by the Environmental Protection Agency (EPA). Alternatives to methylene chloride are available as glycol ethers. Photoresist removal. Dry-film resists have been formulated for ease of removal in both aqueous-alkaline and solvent solutions. Strippers of each type are available for both static tank and conveyorized systems. Cold stripper solvent-type formulations are similar to those used on vinyl screen inks in which the primary solvent is methylene chloride.42 Aqueous-alkaline stripping results in undissolved residues of softened resist films. These residues can be captured in a filter system and disposed of in accordance with waste disposal requirements. Negative-acting, liquid-applied photoresist can be readily removed from printed boards that have not been baked excessively. Baking is critical to removal because it relates to the degree of polymerization.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
94
Chapter Two
Since overbaking is also damaging to the insulating substrates, processes should stress minimal baking—only enough to withstand the operations involved. The negative-acting resists are removed by using solvents and commercial strippers. In this case, the resist does not dissolve; instead, it softens and swells, breaking the adhesive bond to the substrate. Once this has taken place over the entire coated area, a water spray is used to flush away the film. Positive-acting photoresists are removed by dissolving in acetone, ketone, cellusolve acetate, or other organic solvents. Commercial organic and inorganic strippers are suitable if baking has not been excessive. Removal by exposure to UV light and subsequent dipping in sodium hydroxide, trisodium phosphate (TSP), or other strong alkaline solutions is also effective. Overbaking also makes removal difficult. Machine stripping is done in a solution of 0.5 N sodium hydroxide, nonionic surfactants, and defoamers. 2.4.4.3 Etching solutions. This section is a survey of the technology and chemistry of the copper etching systems in common use. Changes from batch-type operation to continuous constant-rate systems with increased process automation represent major innovations in etching practices. Problems encountered in the control of equipment and etchant solutions are frequently difficult to separate. Often, the utmost in performance and life of the etchant is not attained. A current understanding is needed in the areas of fine-line production, regeneration and recycling of materials, and pollution control. Alkaline ammonia. Alkaline etching with ammonium hydroxide complexing is increasingly used because of its continuous operation, compatibility with most metallic and organic resists, minimum undercut, high capacity for dissolved copper, and fast etch rates. Both batch and continuous (closed-loop) spray machine systems are in use. Continuous operation provides constant etch rates, high work output, ease of control and replenishment, and improved pollution control. However, costs are relatively high, neutralization after etching is critical, and the ammonium ion introduced into the rinses presents a difficult waste treatment problem. Complete regeneration with chemical recycling is not routinely practiced. Sulfuric acid–hydrogen peroxide. Sulfuric-peroxide systems are used extensively for copper surface preparation (microetching), i.e., for oxide coating of inner layers, and for electroless and electrolytic copper plating. The reasons for this wide acceptance are the ease of replenishment, simple waste treatment needed, closed-loop copper recovery, and optimum surface texture of the copper. In addition to these advantages, the compatibility of these systems with most organic and metallic resists,
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
95
their steady etch rates, and the optimum undercut they provide make them especially suited to be used as final etch step. Both tank immersion and etching systems are commercially available. Continuous processing equipment is also available for the electroplating-throughetching operations. Cupric chloride. Cupric chloride systems are typical of the innovations to achieve closed-loop regeneration, lower costs, and a constant, predictable etch rate. Steady-state etching with acidic cupric chloride permits high throughput, material recovery, and reduced pollution. Regeneration in this case is somewhat complex but is readily maintained. Dissolved copper capacity is high compared with that of batch operation. Cupric chloride solutions are used mainly for fineline multilayer inner details and print-and-etch boards.43 Resists are screened inks, dry film, gold, and tin-nickel. Solder and tin boards are not compatible with cupric chloride etchant. Persulfates. Ammonium, sodium, and potassium persulfates modified by certain catalysts have been adopted for the etching of copper in PC manufacturing. Continuous regenerative systems and a batch system using ammonium persulfate are common. Wide use is made of persulfates as a microetch for inner-layer oxide coating and copper electroless and plating processes. Persulfate solutions allow all common types of resists on boards, including solder, tin, tin-nickel, screened inks, and photosensitive films. Persulfate solutions are not suitable etchants for gold because of excess undercut and low etch factors. Formulations of ammonium persulfate catalyzed with mercuric chloride have etch rates comparable to those of the chloride etchants and are preferred for solder, print-and-etch, and tin-nickel boards. Formulations with proprietary additives other than mercury catalysts are available and have been improved to give good etch factors. Regenerative systems have made possible higher copper capacities and constant etch rates. In general, persulfate etchants are unstable and will exhibit decomposition, lower etch rates versus copper content, and lower useful copper capacity. The use of persulfate etching systems has declined recently because of high costs and other improvements in alkaline ammonia etchants. Ferric chloride. Ferric chloride solutions are used as etchants for copper, copper alloys, Ni-Fe alloys, and steel in PC applications, electronics, photoengraving arts, and metal finishing. Ferric chloride is used with screen inks, photoresist, and gold patterns, but it cannot be used on tin-lead or tin-plated boards. However, ferric chloride is an attractive spray etchant because of its low cost and its high holding capacity for copper.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
96
Chapter Two
The composition of the etchant is mainly ferric chloride in water, with concentrations ranging from 28 percent to 42 percent by weight (see Table 2.25). Free acid is present because of the hydrolysis reaction. This HCl is usually supplemented by additional amounts of HCl (up to 5 percent) to hold back the formation of insoluble precipitates of ferric hydroxide. Commercial formulations also contain wetting and antifoam agents. The effects of ferric chloride concentration, dissolved copper content, temperature, and agitation on the rate and quality of etching have been reported in the literature.41 Commercial availability includes lump FeCl3⋅6H2O and aqueous solutions with and without additives. Ferric chloride with additives has the advantage of low foaming (reduced odor and fuming), fast and even etching (due partly to added strong oxidizers and surface-wetting properties), and reduced iron hydroxide precipitate formation, owing to the slight acidity and to the chelating additives. The useful life of ferric chloride etchants and the uniformity of etching rates have been greatly improved by the manufacturers of proprietary solutions. Chromic-sulfuric acids. These etchants for solder- and tin-plated boards were preferred for many years. More recently, their use has been limited drastically because of the difficulty in regeneration, the inconsistent etch rate, the low limit of dissolved copper (4 to 6 oz/gal), and especially the pollution concerns. Chromic acid etchant is suitable for use with solder, tin-nickel, gold, screened vinyl lacquer, and dry or liquid film photoresists. Although chromic acid etchants are strong oxidizing agents, they do not attack the solder, since insoluble lead sulfate is formed. Undercut is seen less with solder-plated patterns than with gold and organic resists. Nitric acid. Etchant systems based on nitric acid have not found extensive application in PC manufacture. Copper etching is very exothermic, which may lead to violent runaway reactions. Problems with this system include solution control, attack on resists and substrates, and toxic gas fuming. However, nitric acid has certain advanTABLE 2.25
Composition of FeCl3 Solutions Low strength
Percent by weight Specific gravity Baumé lb/gal g/L Molarity
28 1.275 31.5 3.07 365 2.25
Optimum 34 1.353 38 3.9 452 2.79
38 1.402 42 4.45 530 3.27
High strength 42 1.450 45 5.11 608 3.75
Data taken at 68–77°F (20–25°C). Photoengraving FeCl3 42° Baumé has 0.2–0.4% free HCl. Proprietary etchants contain up to 5% HCl.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
97
tages. These include rapid etching, high dissolved copper capacity, high solubility of nonsludging products, easy availability, and low cost. 2.4.4.4 Equipment and techniques. Etching techniques and the equipment used today have evolved from four basic etching methods: immersion, bubble, splash (paddle), and spray etching. Spray etching is the most common method, since it is fast, well suited to high production, and capable of very fine line definition. Spray techniques include single- and double-sided etching with either horizontal or vertical positioning of the boards. These techniques yield high etch factors and short etching times, due in part to high solution controls and to the introduction of high quantities of air. As in all etching procedures, however, the highest definition (fine-line patterns) or the use of thicker copper foils requires control of the undercutting by careful selection of equipment and etchants. Spray-etching machines have evolved simultaneously with the availability of chemical-resistant metals and plastics essential to their construction (polyvinyl chloride [PVC] and titanium alloys). Titanium is suitable for constant use in all common etchants except sulfuric acid–hydrogen peroxide, which requires stainless steel materials. Polycarbonate, polypropylene, and Hastelloy C alloys are also used. Automatic vertical etching. This type of machine is designed for higher production rates. A mechanism carries a loaded rack through the etch chamber, where it is sprayed on one or both sides by oscillating banks of spray nozzles. The rack goes through water (spray-rinse) and neutralizing chambers. Cooling coils are available for sulfuric-peroxide etchants. Control of pressure to each bank of spray nozzles and on-off valves provide additional versatility. The etchant sump has a larger volume of etchant than drawer-type vertical etchers, as well as a capability for continuous replenishment. Fine-line etching is attainable when spray nozzles, pressure, speed, and other variables are working optimally. Horizontal etching. Double-sided horizontal etchers are generally preferred in PC manufacturing, since the majority of the boards are twosided. The etcher is available with a drawer-type holding rack and also has a built-in sink at the left of the chamber. The etch operation proceeds and automatically pushes the rack into the rinse area after a timed cycle. Etching is done via independently controlled spray-nozzle banks at the top and bottom. Automatic horizontal etching machines. Made for high-volume production, these machines incorporate the features previously listed for horizontal machines, plus the advantages of conveyorized loading and han-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
98
Chapter Two
dling of boards up to 36 in. wide and of indefinite length, as well as built-in rinsing and neutralizing. In operation, machines are loaded by laying boards flat on an open horizontal conveyor belt that carries them progressively through the etch chamber and subsequent rinses. Rollers on conveyor belts are spaced so as to allow the bottom spray to reach the board. Automatic equipment is available for flow-through solution replenishment, which gives constant etch rates. 2.5 Solder Resist Materials and Processes IPC-T-50b defines a solder resist (mask) as “a coating material used to mask or to protect selected areas of a printed circuit board (PCB) from the action of an etchant, solder, or plating.” A somewhat more useful working definition for a solder resist is as follows: a coating that masks off a printed circuit board surface and prevents those areas from accepting any solder during reflow or wave soldering processing (see Fig. 2.25). The prime function of a solder resist is to restrict the molten solder pickup or flow in those areas of the PCB, holes, pads, and conductor lines that are not covered by the solder resist. PCB designers, however, often expect more functionality out of the solder resist than just a means to restrict the solder pickup. Table 2.26 lists the functions of a solder resist. 2.5.1 Design considerations for solder resists
The design goals for the selection and application of a solder resist should be carefully considered. As with all design goals, one should try to achieve maximum design flexibility, reliability, and functionality at a cost consistent with the required level of system performance. The system’s performance and reliability requirements are the keys in determining the selection process for a solder resist. Critical life-support systems will require different materials and standards than a less critical system such as a video cassette recorder (VCR).
Figure 2.25
Major features of solder resist on a PCB.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
TABLE 2.26
99
Functions of Solder Resists
Reduce solder bridging and electrical shorts Reduce the volume of solder pickup to obtain cost and weight savings Reduce solder pot contamination (copper and gold) Protect printed circuit board (PCB) circuitry from handling damage, i.e., dirt, finger prints, etc. Provide an environmental barrier Fill space between conductor lines and pads with material of known dielectric characteristics Provide an electromigration barrier for dendritic growth Provide an insulation or dielectric barrier between electrical components and conductor lines or via interconnections when components are mounted directly on top of the conductor lines
Table 2.27 outlines some of the factors to consider in the design process when selecting a solder resist. It is not very likely that a single solder resist material or application technique will satisfy all the design considerations that are viewed as necessary. It should also be noted that not all the design factors listed in Table 2.27 carry the same weight or value, so the designer needs to prioritize those design factors, analyze the necessary trade-offs, and then specify the solder resist material and process that gives the best balance of properties or characteristics. 2.5.2 Solder resist selection
The solder resists available are broadly divided into two categories, i.e., permanent and temporary. The breakdown of the solder resist types is shown in Fig. 2.26. The permanent solder resist materials are classiTABLE 2.27
Design Factors for Solder Resists
Criticality of system’s performance and reliability Physical size of PCB Metallization on PCB, i.e., SnPb, copper, etc. Line and space (density) of PCB Average height of conductor line (amount and uniformity of the metallization) Size and number of drilled PTHs Annual ring tolerance for PTHs Placement of components on one or both sides of PCB Need to have components mounted directly on top of conductor line Need to tent via holes in order to keep molten solder out of selected holes Need to prevent flow of solder up via holes, which may have components sitting on top of them Likelihood of field repair or replacement of components Need for solder resist to be thick enough to contain the volume of solder needed to make good solder connections Choice of specifications and performance class that will give the solder resist properties that are necessary to achieve design goals
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
100
Chapter Two
Figure 2.26
Solder resist selection considerations.
fied by the means used to image the solder resist, i.e., screen printing or photoprint. In addition, the screen-printed resists are further classified by the curing technique, i.e., thermal or UV curing. The photoprint solder resists are distinguished from each other by whether they are in the form of liquid or dry film. The temporary resist materials are classified by chemistry or means of development. 2.5.2.1 Temporary resists. A distinction is made between permanent and temporary solder resists. The temporary resists are usually applied to a selected or limited area of a PCB to protect certain holes or features such as connector fingers from accepting solder. The temporary resist keeps solder out of the selected holes and thus allows for certain process- or temperature-sensitive components to be added manually at a later time. The temporary solder resists usually consist of a latex rubber material or any of a variety of adhesive tapes. These materials can be applied by an automatic or manual dispenser. Some of the temporary mask materials dissolve in the solvents or cleaning processes that are used to clean off the soldering flux residues. This is really a benefit, since it eliminates the need for a separate manual removal and/or cleaning step for the temporary resist. 2.5.2.2 Permanent resists. Permanent solder resists are not removed and thus become an integral part of the PCB. The demand for permanent solder resist coatings on PCBs has greatly increased as the trend toward surface mounting and higher circuit density has increased. When the conductor line density was low, there was little concern about solder bridging, but as the density increased, the number and complexity of the components increased. At the same time, the incidence of soldering defects, such as line and component shorts, greatly increased. Inspection, testing, and rework costs accelerated as effort went into locating and repairing the offending solder defects. The additional cost of the solder resist on one or both sides of the PCB was viewed as a cost-effective means to offset the higher inspection, testing, and rework costs. The
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
101
addition of a solder resist also had the added value for the designer of providing an environmental barrier on the PCB. This feature was important and dictated that the materials considered for a permanent solder resist should have similar physical, thermal, electrical, and environmental performance properties to the laminate material. See Table 2.28 for a comparison of properties for permanent solder resist types. 2.5.2.3
Selection factors
General considerations ■
Reliability and performance data on the solder resist material
■
Cost effectiveness
■
Past experience
■
Vendor reliability and technical support
■
Number of panels required
■
Appearance and cosmetics of solder resist
■
Number of sources for application and supply Material considerations
■
IPC-SM-840 class designation callout
■
Cost and availability of materials
TABLE 2.28
Permanent Solder Resist Selection Guide Screen print
Feature Soldering performance Ease of application Operator skill level Turnaround time Inspectability Feature resolution Adhesion to SnPb Adhesion to laminate Thickness over conduct or lines Bleed or residues on pads Tenting or plugging of selected holes Handling of large panel size with good accuracy Meeting of IPC-SM-840 Class 3 specification Two-sided application Capital equipment cost
Dry film
Thermal
UV
Aqueous
Solvent
Liquid photoresist
1 1 2 2–3 2–3 3 1 1 3–4
1 1 2 2–3 2–3 3 3 1–2 3–4
1 2 2 2 3 1 1–2 1 1–2
1 2 2 2 3 1 1–2 1 1–2
1 2 2 2 3 1 1 1 2
3–4 4
3 4
1 1
1 1
1 4
3
3
1
1
1
3–4
3–4
1–2
1
1
4 4
4 4
1 1–2
1 1–2
3–4 1
1 = good or high; 2 = moderate; 3 = fair; 4 = poor or low.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
102
Chapter Two
■
Lot-to-lot consistency record
■
Setup and cleanup times
■
Working time and shelf life of solder resist
■
Safety concern for release of noxious or toxic fumes during processing or curing steps
■
Degree of workability Process considerations
■
Operator skill level requirement
■
Need for special applications or curing equipment
■
Cleaning requirements for PCB before and after application
■
Size of PCB
■
Need for solder resist on one or both sides of PCB
■
Number of panels to be processed
■
Turnaround time required
■
Machinability
■
Need to tent selected holes
■
Touchup or rework limitations
■
Inspectability and conformance to specification Performance considerations
■
Testing to IPC-SM-840 specification requirements
■
Adhesion after soldering and cleaning
■
Bleed-out of resist onto pads or PTHs
■
Solvent resistance to flux and flux cleaners
■
Ionic contamination levels
■
Integrity of resist after soldering and thermal cycling
2.5.3 Solder mask over bare copper (SMOBC)
SMOBC is a major solder resist application technology. A problem for conventional copper-tin-lead electroplated PCBs is the flow of tin-lead solder under the solder resist during the wave or vapor phase or infrared soldering. This flow of molten metal underneath the resist can prevent the resist from adhering to metal or laminate. If the resist fractures because of this hydraulic force, the surface integrity is lost and the effectiveness of the resist as an environmental or dielectric barrier can be severely impaired. In fact, such breaks in the resist can actually
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
103
trap moisture, dirt, and soldering flux and serve as a conduit to direct liquids down to the resist-laminate interface. This solder resist situation could lead to serious reliability and/or performance concerns. The SMOBC process addresses the tin-lead flow problem by eliminating the use of tin-lead electroplating on the conductor lines under the solder resist. An all-copper PTH printed circuit board is often produced by a tent-and-etch process. This process is one in which the PCB is drilled and plated with electroless copper, which is immediately followed by copper panel plating with the full-thickness copper required for the PTHs. A dry-film resist process is often used with a negative phototool (clear conductor lines and pads) to polymerize the resist in only those clear areas of the phototool. This polymerized resist will now protect the lines and PTHs during a copper-etching process that will remove all the unwanted background copper. The photoresist is then stripped off, and the solder resist material is applied and processed through curing. Tin-lead is next added to the open component pads and PTHs by the hot-air leveling process. An alternative process uses conventional procedures to create a pattern-plated board. After etching, however, the metal etch resist is removed chemically, leaving the underlying copper bare. Subsequent process steps are the same as for SMOBC. The primary function of tin-lead in the PTHs and on the component pads is to improve solderability and appearance. It is important to demonstrate the solderability of the holes and pads on the SMOBC panel. This is accomplished by a hot-air leveling process that places a thin coating of molten tin-lead on only those copper areas of the PTH that have not been covered by the solder resist. This hot-air leveling process improves the ability of the copper surface to be soldered and also improves the appearance and solderability after longer-term storage of the PTHs and pad surfaces. Since there is no flowable metal under the solder resist during the hot-air leveling step or later during component soldering, the resist maintains its adhesion and integrity. The lower metallization height of the conductor lines allows the use of a thinner dry-film resist and also makes the liquid and screen-printing application somewhat easier. One variation on the basic SMOBC process is to make the PCB by the conventional pattern-plate copper and tin-lead process followed by etching of the background copper. Then another photoresist step is used to tent the holes and pads so that the tin-lead can be selectively stripped from the conductor lines. This is followed by infrared or oil reflow, cleaning, and application of solder resist. A second process variation strips off the tin-lead plating completely and is followed by cleaning, solder resist application, and hot-air leveling. There are still other PCB fabricators that do not like either of these processes and are opt-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
104
Chapter Two
ing to use a nonflowable, copper-etchant-resistant metal like tin-nickel under the solder resist. The major shortcoming of tin-nickel is that it is considered more difficult to solder with low-activity soldering fluxes. 2.5.4 Cleaning and PCB preparation prior to solder resist application
Optimum solder resist performance and effectiveness can be obtained only if the PCB surfaces are properly prepared prior to the application of the resist. Surface preparation usually consists of a mechanical brush scrubbing for the non-tin-lead PCBs followed by an oven-drying step. The tin-lead PCBs should not be scrubbed and require less aggressive cleaning procedures. The cleaning options prior to solder resist application are shown in Table 2.29. Dry-film and liquid-photopolymer resists applied to meet the IPCSM-840 Class 3 requirements are particularly sensitive to the cleaning processes and baking step used to remove volatiles prior to the application of the resist. Tin-lead-coated PCBs should not be mechanically brush-scrubbed because of the smearing potential of such a malleable metal as tinlead. Scrubbing can cause a thin smear of the metal to be wiped across the substrate, leaving a potentially conductive path or, at a minimum, a decrease in the insulation resistance between the conductor lines. Pumice scrubbing is also unacceptable for tin-lead circuitry, since the pumice particles may become embedded in the soft metal, which can lead to poor soldering performance. Solvent degreasing with Freon or 1,1,1-trichloroethane cleaners is necessary with tin-lead PCBs in order to remove the light process oils from the solder reflow step, dirt, and fingerprints that are usually found on the PCB at the solder resist step. Solvent degreasing will not remove metal oxides or contaminates that are not soluble in the degreasing media. The last step prior to the application of a solder resist to the PCB should be an oven-drying step in which absorbed surface moisture and low-boiling volatiles are removed. This drying step should immediately precede the resist application step in order to minimize the reabsorption of moisture. TABLE 2.29
Preparation for Solder Resists Panel metallization
Operation
Cu
Sn-Pb
Others
Mechanical brush Pumice Solvent degrease Chemical cleaning Oven drying
Yes Yes Yes Yes Yes
No No Yes Yes Yes
Yes Yes Yes Yes Yes
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
105
The most stringent performance specifications will in turn require the most stringent cleaning procedures prior to the resist application. Not all resists and performance specifications require the same degree of cleaning. In certain cases, where performance requirements are less stringent, some screen-printed resists may be used successfully without any particular cleaning or oven-drying steps. 2.5.5 Solder resist applications
Permanent solder resists may be applied to the PCB by any of several techniques or pieces of equipment. Screen printing of liquid solder resists (ink) is the most common; with regard to photoprint solder resists, the dry-film solder resists are applied to one or both sides of the PCB by a special vacuum laminator, and the liquid-photoprint solder resists are applied by curtain coating, roll coating, or blank-screenprinting techniques. 2.5.5.1 Screen printing. Screen printing is typically carried out in manual or semiautomatic screen-printing machines using polyester or stainless steel mesh for the screen material. If solder resist is required on two sides, the first side is coated and cured or partially cured and then recycled to apply the solder resist on the second side using the screen pattern for that side, and then the entire PCB is fully cured. 2.5.5.2 Liquid photoprint. For some liquid-photoprint solder resists, a screen-printing technique is used to apply the resist in a controlled manner to the surface of the PCB. The screen has no image and serves only to control the thickness and waste of the liquid solder resist. There is no registration of the screen, since there is no image. The actual solder resist image will be obtained by exposing the coated PCB using ultraviolet light energy and the appropriate phototool image. The unexposed solder resist areas defined by the phototool are washed away during the development step. Some liquid-photoprint solder resists require a highly mechanized process (roller or curtain coating) and therefore, because of the equipment costs and the setup, cleanup, and changeover costs, are best suited to high-volume production. The liquid solder resists do not tent holes as effectively as the dry-film solder resist materials. 2.5.5.3 Dry film. Dry-film solder resists are best applied using the vacuum laminators that have been designed for that purpose. The equipment removes the air from a chamber in which the PCB has been placed. The solder resist film is held out of contact from the PCB surface until atmospheric pressure is used to force the film onto one or both sides of the PCB.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
106
Chapter Two
The roll laminators that apply the dry-film resists for plating or etching are usually found to be unacceptable for solder resist application. The roll laminators were designed to apply a resist to a smooth, flat surface such as copper foil, and not to a three-dimensional surface such as an etched and plated PCB. Air is usually trapped adjacent to the conductor lines as the lamination roll crosses over a conductor line running parallel to the lamination roll. Entrapped air next to the conductor lines can cause wicking of liquids, which in turn causes reliability and/or performance concerns. The dry-film resist thickness, as supplied, is usually 0.003 or 0.004 in. and will meet the requirement of the Class 3 specification for a 0.001-in. minimum thickness of solder resist on top of the conductor lines. The resist thickness chosen depends on the expected thickness of the copper circuitry to be covered, allowing for filling of the spaces between circuit traces with resist. 2.5.6 Curing
Once the solder mask has been applied to the PCB, it must be cured according to the manufacturer’s recommendations. Typically, curing processes include thermal curing by oven baking or infrared heating, UV curing, or a combination of the two processes. The general objective of the curing process is to remove any volatiles (if present) and to chemically cross-link and/or polymerize the solder resist. This curing toughens the resist to help ensure that it will maintain its integrity during the chemical, thermal, electrical, and physical exposure the PCB will see during its service life. Undercuring, or an out-of-control curing process, is usually the prime cause for solder resist failure. The second leading cause for failure is inadequate cleaning prior to solder resist application. All PCBs should be carefully inspected for defects prior to curing. Once a solder resist has been cured, it is usually impossible or impractical to strip the resist for rework without seriously damaging the PCB. 2.5.7 Liquid photoimageable solder resist (LPISR)
With the advent of SMT in the early 1980s, the requirements for tighter registration of solder mask to circuit features have become ever more demanding. As the lead pitch of SMT components became finer, as illustrated in Table 2.30, conventional thermal and UV-curable screen resists could no longer satisfy the requirements to deposit material completely and consistently between the board features, such as adjacent traces or traces and pads. Although dry-film solder resist (DFSR) is able to satisfy many of these tighter tolerance requirements, it is expensive and sometimes it has difficulty in coverage of spacings
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
TABLE 2.30
107
Standard Design Rules for Surface Mount Device Pads (mm) Pad
Kind of SMD
Number of pins
Pitch
SOP (PLCC)
8–28
1.27
QFP
64 80 100 48 224 300
1.0 0.8 0.65 0.5 0.4 0.3
Solder mask
Width
Space
Clearance
Width
0.5–0.6
0.77–0.67
0.1–0.15
0.37–0.57
0.6–0.7
0.67–0.57
0.1–0.15
0.27–0.47
0.6 0.5 0.35 0.3 0.22 0.15
0.4 0.3 0.3 0.2 0.18 0.15
0.135 0.085 0.085 0.05 0.05 0.04
0.2 0.13 0.13 0.1 0.08 0.07
PLCC: plastic leaded chip carrier. SOURCE: NEC Corporation.
between tightly formed fine-line conductors at their base area, leaving small air pockets that tend to erupt during the soldering operation. Therefore, the use of DFSR has declined as SMT has proliferated and LPISR has gained acceptance. The usage of DFSR seems to be confined to some special cases when requirements such as hole tenting, small lot size, and thicker mask (3 mil or more) are present. When Ciba-Geigy introduced the Probimer 52 LPISR system in 1978, SMT was not yet in place and most of the PCB manufacturers were reluctant to adopt it because the cost of the Probimer system was expensive compared to what they were then using. However, some PCB manufacturers catering to the telecommunication industry started to adopt it because of its excellent corrosion resistance; then, as SMT started to gain momentum in the mid-1980s, other solder resist ink makers saw the value of LPISR and followed Ciba-Geigy into the marketplace. Today, there are a great number of LPISR manufacturers offering material and process alternatives, and nearly all SMT boards are coated with LPISR. 2.5.7.1 Panel preparation. Before proceeding with the topic of coating methods, a discussion of panel preparation is appropriate because it is the starting point of all processes. When cleaning copper circuitry for solder mask application, it is important to remove all intermetallic compounds, oxides, and organic and ionic contaminants. A typical cleaning process may consist of the following steps: ■
Acid spray rinse (5 percent hydrochloric acid, for example)
■
Water spray rinse
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
108
Chapter Two
■
Mechanical abrasion (jet scrub, pumice scrub, brush scrub, etc.)
■
High-pressure water and deionized water rinse
■
Dry and optional bake at about 160 to 180°F for 30 min
Mechanical abrasion ensures better adhesion of solder resist to copper and helps resist ink to flow into spacings more naturally by removing sharp conductor edges that sometimes block the smooth flow of resist ink. 2.5.7.2 Screen coating. Open screen coating is the simplest entrylevel method for most PCB manufacturers, although screen coating can be very sophisticated when the process is to be automated. Single-sided screen coating. On a worldwide basis, the most popular coating method by far is single-sided open screen coating because it is relatively easy to do successfully and has a low entry cost. By its nature, however, screen coating tends to remove resist ink at the conductor edge that makes the first contact with the squeegee and leave spacings between densely spaced conductors uncovered, whether it is single-sided or the simultaneous double-sided coating to be explained in the next subsection. (Figure 2.27 shows this weakness.) To overcome this weakness, the users of the screen-coating method normally screen the panel twice or even three times to ensure sufficient coverage at conductor edges and spacings, particularly at their bottom area. Users of PCBs usually demand that the thickness of the solder resist be about 0.6 mil (or 0.15 mm) at the edges of the conductors. Simultaneous double-sided screen coating. This method was conceived by a Japanese PCB manufacturer, Satosen, and the hardware implementation was made by another Japanese company, Toshin Kogyo. Depending on the models, double-sided screening equipment can coat between 120 and 180 panels per hour. These screening machines are equipped with back-side scrapers to prevent resist ink from falling into holes.
Figure 2.27
“Skipping” problem associated with screen coating.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
109
There is another maker of double-sided screening equipment: Circuit Automation. The equipment made by this company is essentially the same as the Japanese machine. However, the Circuit Automation machine, sold under the trade name of DP series, avoids ink getting into holes by moving the screen slightly and changing the skew angle of the squeegee on the second screening. Double-sided screen coating advantages/disadvantages. One major advantage of the double-sided simultaneous screening method is that the panel receives tack-free curing only once, and therefore the degree of cure on both sides of the panel is equal. Single-sided screening makes the first side cure more than the second side, and, in some extreme cases, the colors of the two sides may become different. Double-sided screen coating has one weakness in that it is difficult to screen thin panels. To overcome this problem, the makers of such equipment provide a special frame on which to mount thin panels, which gives tension to the panel and makes screening possible. However, the throughput by the thin-panel version is somewhat reduced due to the more intricate panel-mounting scheme.
2.5.7.3 Curtain coating. Ciba-Geigy introduced the first curtain coating system, the Probimer 52, in 1978. Coates Circuit Products of the United Kingdom followed. Years later, Maas of Germany started to offer curtain-coating equipment, but no resist ink. Figure 2.28 shows a typical fully automated configuration of a curtain-coater line.
Dryer
Coater
Turn-over device (not shown)
Cart
Dryer
vel Tra yor e v n Co
Coater
Cart
Figure 2.28
Typical fully automated configuration of a curtain-coater line.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
110
Chapter Two
The speed of the belt conveyor under the curtain of resist ink determines the thickness of the coating. One pass is sufficient to secure the required coating thickness. The quality of coverage by curtain coating is excellent. Curtain coating can accommodate mixed panel sizes of different thicknesses without any setup change, but it can coat only one side of the panel at a time. Because of the nature of coating, the entire panel surface gets coated. To provide room for tooling holes and test coupons, 15 to 25 percent of the panel area is used as trimming, and resist ink coated on this trimming area is wasted in curtain coating. That is, “useful” ink utilization in curtain coating is usually between 75 and 85 percent. However, the newer curtain coaters have the provisions to block two edges of the panel from being coated, thus improving resist ink utilization. In the early days of curtain coaters, it was difficult to coat thin panels since the leading edge of a thin panel tends to droop down at the end of the fast conveyor belt under the curtain. However, this problem is overcome by a flipping mechanism provided at the end of the conveyor belt. To avoid the “lap-around” effect of resist ink at the leading edge of the panel, the panel is usually fed into the curtain at a slightly skewed angle. Curtain coating can process typically 180 panels per hour; a high-productivity model can handle in excess of 300 panels per hour. The process after coating is more or less the same as in screen coating. Newer types of tack-free curing ovens are made much shorter than the original one, and the entire length of a fully automated line with two curtain coaters in series is no more than 60 to 70 ft. 2.5.7.4
Spray coating
When it comes to the arrangement of spray guns (atomizers), there are also a few variations. In one variation, a single gun sways sideways back and forth, perpendicular to the direction of panel travel. In a second single-gun system, the gun is stationary. In other coaters, two stationary guns are arranged in staggered position. Each one of these gun arrangements has its strength and weaknesses. In electrostatic spray systems, effective grounding is essential for good results. Also, it is important to keep a distance of about half an inch between adjacent panels. If the adjacent panels get closer than this clearance, sparks may be induced at the edges of these panels, leaving uncoated spots. In such a system, the typical coating speed is about 240 panels per hour. Vertical spray systems.
Horizontal spray systems. All horizontal systems coat one side at a time. In most such systems, the panel is tack-free cured before being coated
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
111
on the second side. In some systems, however, the panel is carried on a V belt. After the first side is coated, the panel is flipped and the other side gets coated. In this case, tack-free curing is done only once, but it is difficult to process thin panels in such a system. Thin panels are usually spray coated vertically. Overspray. Unlike screen and curtain coating, spray coating creates an overspray. There are various ways to treat oversprayed ink. In one system, a roll of paper 800 to 1000 yards long is used to absorb oversprayed ink. When the entire length of paper is used up, it is removed and treated for waste disposal. In other systems, a container tank is provided underneath the carrying belt to collect oversprayed ink. When the tank gets filled to a certain level (about once every two to three months), chemicals are added to coagulate the ink, and the coagulated ink is carted away for waste disposal. Curtain-coating and spray-coating methods can process panels of different sizes and shapes without special setup, which is an advantage in dealing with small lot sizes. On the other hand, when panels of mixed sizes are passed through a spray coater, ink utilization can be very poor—as low as 40 percent. Some resist ink manufacturers claim oversprayed ink can be used again by adding solvent, but in reality, reutilization of oversprayed ink is not done because such solvents are not a part of ink formulation and are not compatible with the main ingredients. Spray coating gives the best conformal coverage on the peaks and valleys of the panel surface. Because of this, however, spray coating can create skips in subsequent legend screening when valleys are too low, as illustrated in Fig. 2.29. After years of struggle, ink makers have now corrected this “skipping” problem by formulating spray inks to fill the valleys high.
2.5.8 Tenting holes
All coating methods described so far have one problem in common. None of the methods can effectively and reliably tent holes. Closely
Figure 2.29 Spray coating can create good conformity with circuits, which, however, may cause skipping problems in legend screening.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
112
Chapter Two
placed feed-through holes can cause bridging at the time of soldering. Flux can be entrapped in small holes. Therefore, some users of PCBs demand that the holes be tented or filled with solder mask. Dry-film solder mask can provide tenting, but it is usually expensive and often fails to fill the narrow valleys between tightly spaced conductors. To overcome this difficulty, DuPont came up with a solution with the VALU system, in which the panel is first coated thinly with LPISR and then dry-film solder mask is laminated on top of it. When hole tenting is required in conjunction with screen, curtain, or spray coating, holes are filled with epoxy-based ink by screening after the panel is coated with LPISR. Some PCB manufacturers fill the holes first before coating with LPISR. Such processes add extra cost, but there seems to be no better alternative way to accomplish hole tenting. 2.5.9 Electroless Ni/Au plating issues for solder resists
Hot-air solder leveling (HASL) is the most popular surface finish for SMT. As the density of SMT boards becomes higher, first-pass assembly yields tend to be poorer and repair is very costly and error prone. In recent years, electroless nickel-gold finish has been gaining popularity as an alternative finish to HASL. MLBs for cellular telephone applications and a large portion of Personal Computer Memory Card International Association (PCMCIA) cards (now called PC cards) are finished with electroless Ni-Au plating, which provides excellent protection against oxidation before the soldering operation. Boards with Ni-Au finish can withstand a few soldering cycles without oxidation. Initially, some LPISRs could not withstand the electroless Ni-Au plating operation. Improvements have been made on most LPISRs available in the market to accommodate electroless Ni-Au plating. If a given LPISR is not suitable for electroless Ni-Au plating, LPISR makers offer versions of their resist inks that can satisfy the plating requirement. 2.6 Machining and Routing Laminate machining consists of the mechanical processes by which circuit boards are prepared for the vital chemical processes of image transfer, plating, and etching. Such processes as cutting to size, drilling holes, and shaping have major effects on the final quality of the printed board. This section will review the basic mechanical processes that are essential to producing the finished board. 2.6.1 Punching holes (piercing) 2.6.1.1 Design of the die. It is possible to pierce holes down to one-half the thickness of XXXPC and FR-2 laminates and one-third that of FR-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
113
3 (Fig. 2.30). Many die designers lose sight of the fact that the force required to withdraw piercing punches is of the same magnitude as that required to push the punches through the material. For that reason, the question of how much stripper-spring pressure to design into a die is answered by most toolmakers: “as much as possible.” When space on the dies cannot accommodate enough mechanical springs to do the job, a hydraulic mechanism can be used. Springs should be so located that the part is stripped evenly. If the board is ejected from the die unevenly, cracks around holes are almost certain to occur. The bestquality holes are produced when the stripper compresses the board an instant before the perforators start to penetrate. If the stripper pressure can be made to approach the compressive strength of the material, less force will be required and the holes will be cleaner. If excessive breakage of small punches occurs, determine whether the punch breaks on the perforating stroke or on withdrawal. If the retainer lock is breaking, the cause is almost certain to be withdrawal strain. The remedy is to grind a small taper on the punch, no more than 11⁄2 in. and to a distance no greater than the thickness of the material being punched. If the grinding is kept within those limits, it will have no measurable effect on hole quality or size. The other two causes of punch breakage are poor alignment, which is easily detected by close examination of the tool, and poor design, which usually means that the punch is too small to do the job required. 2.6.1.2 Tolerance of punching holes. If precise hole size tolerance is required, the clearance between punch and die should be very close; the die hole should be only 0.002 to 0.004 in. larger than the punch for paper-based materials (Fig. 2.31 and Table 2.31). Glass-based laminates generally require about one-half that tolerance. Dies have, however, been constructed with as much as 0.010 all-around clearance between punch and die. They are for use where inspection standards permit rough-quality holes.
Proper sizing and locating of pierced holes for paper laminates.
Figure 2.30
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
114
Chapter Two
Figure 2.31 Proper tolerance of a punch and die.
A die with sloppy clearances is less expensive than one built for precision work, and wide clearance between punch and die causes correspondingly more breakage and less shear than a tight die will cause. The result is a hole with a slight funnel shape that makes insertion of components easier. Always pierce with the copper side up. Do not use piercing on designs with circuitry on both sides of the board, because lifting of pads would probably occur. 2.6.1.3 Hole location and size. Designs having holes whose distance from the edge of the board or from other holes approaches the thickness of the material are apt to be troublesome. Such designs should be avoided; but when distances between holes must be small, build the best die possible. Use tight clearance between punch and die and punch and stripper, and have the stripper apply plenty of pressure to the work before the punch starts to enter. If the distance between holes is too small, cracks between holes may result even with the best of tools. If cracks between holes prove troublesome, plan the process so that the piercing is done before any copper is etched away. The reinforcing effect of the copper foil will help eliminate cracks. Most glass-epoxy laminates may be pierced, but the finish on the inside of the holes is sometimes not suitable for through-hole plating. 2.6.1.4 Press size. The size of the press is determined by the amount of work the press must do on each stroke. The supplier of copper-clad TABLE 2.31
Tolerances for Punching or Blanking Paper-Based Laminates
Material thickness To and including 1 ⁄16 in. Over 1⁄16 in. to and including 3⁄32 in. Over 3⁄32 in. to and including 1⁄8 in.
Base material
Tolerance on hole size (in.)
Up to 2 in.
2–3 in.
3–4 in.
4–5 in.
Tolerances for blanked parts, overall dimension (in.)
Paper
0.0015
0.003
0.004
0.005
0.006
0.003
Paper
0.003
0.005
0.006
0.007
0.008
0.005
Paper
0.005
0.006
0.007
0.008
0.009
0.008
Tolerances (in.) on distance between holes and slots (90°F)
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
115
sheets can specify a value for the shear strength of the material being used. Typically, the value will be about 12,000 lb/in2 for paper-based laminate and 20,000 lb/in2 for glass-epoxy laminate. The total circumference of the parts being punched out multiplied by the thickness of the sheet gives the area being sheared by the die.
2.6.2 Blanking, shearing, and cutting of copper-clad laminates Blanking glass-based laminates. Odd shapes that cannot be feasibly produced by shearing or sawing are either blanked or routed. Glass blanking is always done at room temperature. Assuming a close fit between punch and die, the part will be about 0.001 in. larger than the die that produced it. The tools are always so constructed that a part is removed from the die as it is made. It cannot be pushed out by a following part, as is often true when the material has a paper base. If material thicker than 0.062 in. is blanked, the parts may have a rough edge. The life of a punch, pierce, or blank die should be evaluated with reference to the various copper-clad materials that may be used. One way to evaluate die wear caused by various materials is to weigh the perforators, or punches, very accurately, punch 5000 pieces, and then reweigh the punches. Approximately 5000 hits are necessary for evaluation, because the initial break-in period of the die will show a higher rate of wear. Also, of course, the quality of the holes at the beginning and end of each test must be evaluated. Greatly enlarged microphotos of the perforator can be used for visual evaluation of changes in the die.
2.6.2.1
2.6.2.2 Shearing. When copper-clad laminates are to be sheared, the shear should be set with only 0.001 to 0.002 in. clearance between the square-ground blades (Fig. 2.32). The thicker the material to be cut, the greater the rake or scissor angle between the top and bottom shear blade. The converse also is true: The thinner the material, the smaller the rake angle and the closer the blades. Hence, as in many metal shears, the rake angle and the blade gap are fixed; the cutoff piece can be twisted or curled. Paper-based material can also exhibit feathered cracks along the edge that are due to too wide a gap or too high a shear angle. This can be minimized by supporting both piece and cutoff piece during the shear operation and decreasing the rake angle. Epoxy-glass laminate, because of its flexural strength, does not usually crack, but the material can be deformed if the blade clearance is too great or the shear angle is too large. As in blanking, the quality of a part produced from paper-based laminates by shearing can be improved by warming the material before performing the operation.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
116
Chapter Two
Figure 2.32
Typical adjustable shear blades for Cu-clad laminates.
2.6.2.3 Sawing glass-based laminates. When glass-based laminates are to be sawn, carbide-tooth circular saws can be used; but unless the volume of work is quite low, the added investment required for diamondsteel-bonded saws will be paid for in future savings. The manufacturer’s recommendation for saw speed should be followed; usually it will be for a speed in the neighborhood of 15,000 ft/min at the periphery of the saw blade. When economics dictate the use of carbide-tooth circular saws for cutting glass, use the instruction previously given for paper-based laminates (see Fig. 2.33 for tooth shape) and remember that each caution regarding runout, vibration, and alignment becomes more important when glass-reinforced laminates are sawn. 2.6.3 Routing
Modern circuit board fabricators rely principally on routing to perform profiling operations. The high cost and extended lead times for blanking dies, combined with the problem of design inflexibility of hard tooling, limit the punching operation generally to very high volumes or designs specific to die applications. Shearing or sawing are limited to
Figure 2.33 Typical saw tooth designs for paper and cloth laminates.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
117
rectangular shapes and generally are not accurate enough for most board applications. In the modern circuit board fabrication industry, rapid response to customer lead times and economies of universal process application are well served by routing, especially multiple-spindle computer numerically controlled (CNC) routing. Routing consists of two similar, yet vastly different fabrication processes: CNC multiple-spindle routing and manual pin routing. The similarities consist of the use of highspeed spindles, utilizing carbide cutting tools, and generating high cutting rates. 2.6.3.1 Pin routing. Pin routing is a manual routing process utilizing a template machined of aluminum, FR-4 laminate, or a fiber-reinforced phenolic. The template is made to the finished board dimensions and has tooling pins installed to register to the board’s tooling holes. The package (which can have up to four pieces in a stack) is routed by tracking the template against a pilot pin protruding from the router table. The pin height is less than the template thickness. Usually, the machine pilot pin is the same diameter as the router bit and can be offset adjusted to give the operator flexibility in optimizing dimensions. Work should be fed against the rotation of the cutter to prevent the cutter from grabbing. Pin routing can be an economical process when a small generation of boards is profiled, or if the shapes required are relatively simple. For pin routing to be effective, generally a very skilled operator is required to fabricate the template and to route the boards. Outside machine shops can build aluminum route fixtures for each customer application; however, lead times and costs per order must be considered. Pin routing is usually used by small shops not able to invest in the CNC equipment and its associated support, or as a specialty process, offline from CNC routing. In the best pin routing operations, the volumes produced cannot be compared with multiple-spindle routing. 2.6.3.2 CNC operation. CNC router equipment has the ability to process high volumes of circuit boards very accurately and economically, yet it is coupled with features to enable quick program and setup. This coupling enables the same processing used for high volume to be utilized for prototypes and short-lead-time production. With circuit board data files so universally available, the part programming time has dropped to a few minutes, as opposed to the hours it once took, while setups remain at about 15 to 20 min, plus cutter labyrinth and first article routing. Router operation consists of multiple spindles (two to five) capable of operating at 6,000 to 36,000 rpm or more. The router path (x-y table
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
118
Chapter Two
movement and spindle plunge and retract) is determined by program. This permits any number of paths and any location. The preferred method of registration of the panel to the machine table is to use the full panel and the tooling holes previously drilled. Tooling holes internal to the part provide for the highest accuracy, although manufacturing panel tooling may be used if considered earlier in the process. 2.6.3.3 Tooling. To simplify tooling and expedite loading and unloading operations, effective hold-down and chop-removal systems should be provided as part of the machine design. Various methods may then be devised to mount the boards to the machine table while properly registering them to facilitate routing the outline. Some machine designs will have shuttle tables available so that loading and unloading may be accomplished while the machine is cutting. Others will utilize quick-change secondary tooling pallets or subplots that allow rapid exchange of bench-loaded pallets with only a few seconds between boards. Tooling plates. Tooling plates utilize bushings and a slot on the centerline of the active pattern under each spindle. They are doweled to the machine table (Fig. 2.34). The plates may be made by normal machine shop practice, or the router may be used to register and drill its own tooling plate. Mounting pins in the tooling plate should be light slip fit. Subplates. Subplates should be made of Benelax, linen phenolic, or other similar material. Subplates should have the pattern to be routed cut into their surfaces. The patterns act as vacuum paths and aid in chip removal. Part-holding pins should be an interface fit in subplates and snug to loose fit in the part, depending on cutting technique used (Fig. 2.35). It is recommended that the programmer generate the tool-
Figure 2.34
Typical tooling of numerically controlled routing.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
119
Tooling schematics for numerically controlled routing.
Figure 2.35
ing and hold-down pinholes in addition to the routing program. That will provide absolute registration between the tooling holes and the routing program. 2.6.4 Scoring
Scoring is a circuit board fabrication method used to make long, straight cuts quickly, and therefore it is often used to create rectangular profile board shapes. More commonly, however, it is used in concert with CNC routing for complex shapes, enabling each tool to be used to its unique advantage. When used with routing, scoring has a much wider application and can provide simple breakaway for complex profiles (Fig. 2.36). 2.6.4.1
Operation. Two major types of panel scoring systems are
available:
Scoring process. (a) Typical scoring lines and routed corners. (b) Scoring lines and routed complex features.
Figure 2.36
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
120
Chapter Two
■
Dedicated CNC scoring machines utilizing high-speed carbide or diamond-embedded cutter blades, operating as a pair, one on each side of the board. This generates the V groove on each side simultaneously.
■
Drills or driller/routers equipped with scoring software and spadetype carbide bits, generating score lines on one side of the panel at a time (Fig. 2.37).
Dedicated scoring equipment. The dedicated CNC scoring machines are high-production, precision computer-driven machines. With an exception or two, they utilize blade-type cutting tools of all carbide or with carbide inserts, as well as diamond-embedded varieties, and are designed to self-center the panel. The panel feed rate is high due to the blade’s ability to operate at highsurface-feet cutting rates. Scoring both sides simultaneously with one pass contributes greatly to elevated production processing. This equipment utilizes pin or edge registration, with positioning of score lines and steps by programmed instructions. The vertical adjustment of the cutter blades permits variation in V groove depth, and on many models jump scoring is available. The ability to do jump scoring, or score/no-score segments along a simple line at desired points, is programmable. Multiple-role machines. Scoring with CNC drillers or driller/router machines equipped with scoring software produces score lines only on one side of the panel per machine cycle, although each spindle can be used. The panel and program data must be flipped to score the second side. The panel registration method is similar to that of routing, using existing tooling holes to pin the panel to the machined tooling plates. The tooling plates must be machined flat to assure uniformity of score depth. Brush-type spindle pressure foot inserts should be used to apply downward pressure during score line cutting. Spade-type carbide tools of various angles and configurations are used in the spindles. Typically, multiple passes (two or three) may be required to produce a clean, uniform score line.
2.6.4.2 Applications. Scoring is accomplished by machining a shallow, precise, V groove into the top and bottom surfaces of the laminate, gen-
Figure 2.37
Double-pin method.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
121
erally with the use of CNC equipment. The two most significant elements of the score line are as follows: ■
The positional accuracy from the reference feature (usually the registration hole)
■
The depth of the score, which determines the web thickness
The final edges of a scored circuit board are yielded by breaking the panel, or border, at the score line (Fig. 2.38). The angle of the cutting tool is reflected in the V groove geometry, and limiting this angle to 30 to 90° will minimize score line intrusion into traces near the edges of the circuit board. The score line exposes the laminate glass fibers and resin. Measurements from these surfaces will vary greatly, even though the score line is precisely machined (Fig. 2.39). These irregular surfaces will be noticed as dimensional growth and should be considered in design or planning when designated as a scored edge. The dimensional accuracy of the final board is determined by the degree of precision with which the following are performed: ■
Misalignment within ⫾0.003 in. of the score line from the desired location
■
Web thickness within ⫾0.006 in. of the designated dimension
Typically, nominal web thickness is 0.020 in. for 0.060-in.-thick FR-4 boards and 0.014 in. for 0.030-in.-thick FR-4 laminate. For CEM-1 or CEM-3 materials, 0.040-in. and 0.024-in. nominal web thicknesses apply, respectively. These web thickness values enable sufficient module strength to avoid accidental or premature score separation, while providing simple breaking efforts without excessive edge roughness or growth.
Figure 2.38
Cross section of boards showing finished V grooves and break.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
122
Chapter Two
Figure 2.39
Single-pin method.
2.7 References 1. Coombs, C. F. Jr., Printed Circuits Handbook, 4th ed., McGraw-Hill, New York, 1996. 2. Swiggett, Robert L., Introduction to Printed Circuits, John F. Rider Publisher, Inc., New York, 1956. 3. Senturia, S. D., N. F. Sheppard, H. L. Lee, and S. B. Marshall, “Cure Monitoring and Control with Combined Dielectric Temperature Probes,” Proc. SAMPE, 19(4):22–26, 1983. 4. Kranbuehl, D. E., S. E. Belos, and P. K. Jue, “Dynamic Dielectric Characterization of the Cure Process: LARC-160,” Proc. SAMPE, 19(4):18–21, 1984. 5. Stoll, R., “High Definition Imaging,” PC Fab, 17(6):31, June 1994. 6. Hecht, L., and M. Cibulsky, “Particle Collection Using a Cascade Impactor,” PC Fab, 34, May 1992. 7. Wisnosky, M., “Modeling of Defects in the Print and Etch Process of Printed Circuit Board Manufacturing,” Proc. IEEE Electronic Components & Technology Conference, p. 520, 1986. 8. Moreau, W., Semiconductor Lithography, Plenum Press, New York, pp. 267–281, 1989. 9. Crum, S., “Surface Preparation Process Improvements,” Electronic Packaging & Production, 24, July 1993. 10. Heden, D. J., “Improving Fine Line Resolution with High Intensity Exposure,” PC Fab, 48, December 1987. 11. Deckert, C. A., “Electroless Copper Plating,” ASM Handbook, vol. 5, pp. 311–322, 1994. 12. Murray, J., “Plating, Part 1: Electroless Copper,” Circuits Manufacturing, 25(2):116–124, February 1985. 13. Polakovic, F., “Contaminants and Their Effect on the Electroless Copper Process,” IPC Technical Review, 12–16, October 1984. 14. Blurton, K. F., “High Quality Copper Deposited from Electroless Copper Baths,” Plating and Surface Finishing, 73(1):52–55, 1986. 15. Lea, C., “The Importance of High Quality Electroless Copper Deposition in the Production of Plated-Through Hole PCBs,” Circuit World, 12(2):16–21, 1986. 16. Glasstone, S., Introduction to Electrochemistry, D. Van Nostrand, New York, 1942. 17. Potter, E. C., Electrochemistry, Cleaver-Hume Press, Ltd., London, 1961. 18. Raub, E., and K. Muller, Fundamentals of Metal Deposition, Elsevier, Amsterdam, 1967. 19. Lowenheim, F. A., Modern Electroplating, 3d ed., J. Wiley & Sons, New York, 1974. 20. Safranek, W. H., The Properties of Electrodeposited Metals and Alloys, 2d ed., American Electroplaters and Surface Finishers Society, Florida, 1986. 21. Bard, J., and L. R. Faulkner, Electrochemical Methods: Fundamentals and Applications, J. Wiley & Sons, New York, 1980. 22. Luke, D. A., “Electroplating Copper for Printed Circuit Manufacture,” Circuit World, 13(1):18–23, 1986. 23. Carano, M., “High Speed Copper Plating for Printed Wiring Boards,” Printed Circuit Fabrication, 6(7):1983.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Conventional Printed Circuit Board Technologies
123
24. Sullivan, B., “Electroplating Theory and the High Speed Copper Debate,” Printed Circuit Fabrication, 8(8):35–54, 1985. 25. Mattoon, T. R., P. McSwiggen, and S. A. George, “Printed Circuit Plating Bath Process Control,” Metal Finishing, 83: Parts I, II, and III, 1985. 26. Darikh, P. J., “Electro-deposited Copper for Hi-Rel PCs,” Electronic Packaging & Production, 17(3):61–65, 1977. 27. Jawitz, M. W., “Trouble Shooting Manual for Printed Circuit Production,” Insulation/Circuits, 22(4):5–36, 1976. 28. Strickland, G. R., “Pyrophosphate Copper Plating in Printed Circuit Manufacture,” Product Finishing, 4:20–24, 1972. 29. Rothschild, B. F., “The Effect of Ortho-phosphate in Copper Pyrophosphate Plating Solutions and Deposits,” Metal Finishing, 84(1):49–51, 1978. 30. Dini, J. W., H. R. Johnson, and J. R. Helms, “Effect of Some Variables on the Throwing Power and Efficiency of Copper Pyrophosphate Solutions,” Plating, 54(12):1337, 1967. 31. Rothschild, B. F., “Copper Electroplating Systems: An Evaluation,” Electronic Packaging & Production, 15(8):102–107, 1975. 32. Owen, C. J., H. Jackson, and E. R. York, “Copper Pyrophosphate Plating without Additives,” Plating, 54:821–825, 1967. 33. Hayes, L. E., “Organic Additives for Pyrophosphate Copper: Panacea or Poison?” Electronic Packaging & Production, 17:102–104, 1977. 34. Sherlin, D. E., and L. K. Bjelland, “Improve Electrodeposited Copper with Organic Additives and Baking,” Insulation/Circuits, 24(9):27–32, 1978. 35. Price, J. W., Tin and Tin Alloy Plating, Electrochemical Publications Ltd., AYR, Scotland, 1983. 36. Davis, P. E., and E. F. Duffek, “The Proper Use of Tin and Tin Alloys in Electronics,” Electronic Packaging & Production, 15(7), 1975. 37. Kilbury, R. G., “Producing Buried Via Multilayers: Two Approaches,” Circuits Manufacturing, 25(4):30–49, 1985. 38. Reid, Frank H., and William Goldie, Gold Plating Technology, Electrochemical Publications Ltd., AYR, Scotland, 1974. 39. Ali, H. O., and R. A. Christie, “A Review of Electroless Gold Deposition Processes,” Circuit World, 11(4):10–16, 1985. 40. Goldman, P., et al., “Enhanced SMT Solderability with No HASL: Proprietary Treatments for Copper Pads,” IPC Technical Review, December 1990. 41. Murski, K., and P. M. Wible, “Problem-Solving Processes for Resist Developing, Stripping, and Etching,” Insulation/Circuits, February 1981. 42. Deforest, S., Photoresist Materials and Processes, McGraw-Hill, New York, 1975. 43. Gorman, F., “Regenerative Cupric Chloride Copper Etchant,” Electronic Packaging & Production, 43–46, January 1974.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conventional Printed Circuit Board Technologies
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Source: Microvias
Chapter
3 Microvias by Mechanical Drilling
3.1 Introduction There is a strong global market trend toward handheld devices such as cellular phones and digital personal assistants. While the first challenge was miniaturization and weight reduction, the focus now is on additional features or customer value. Highly prized models combine more and more functions, increasing the complexity of the devices. Examples are integrated cell phones, Internet browsers, global positioning systems, and so forth. This trend coincides with ever shorter product lifetimes and decreasing prices. Hot products used this year will be either obsolete next year, or at best offered at much lower prices. Microvia technology can be successfully applied to achieve higher density and smaller feature sizes. Mechanical drilling covers a wide diameter range while pushing the limits toward smaller via sizes. Conventional mechanical drilling for non-microvias can drill all kinds of PCB materials, such as FR-4, Mitsubishi Gas and Chemical’s BT, General Electric’s GETEK, Hitachi Chemical’s MegTran (FR-4.5), and Matsushita’s MCL-679. There are many equipment vendors supplying various mechanical drilling systems, such as Advanced Controls, ATI, Ching Huei, Datron, Electro Scientific Industries, Inc., Excellon, Hitachi, OZO, Panasonic, Pluritec, Posalux, Sieb & Meyer, Technic, and Yaskawa.1 In general, mechanical drilling is not suitable for forming microvias. However, with innovative technologies of high-speed spindle and numerical control, it is still possible to make small holes at the scale of microvias by mechanical drilling. For instance, Excellon Automation has been developing an NC drilling machine that may form microvias down to 100 µm (4 mil).1 125
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Mechanical Drilling
126
Chapter Three
3.2 Mechanical Drilling for Via Formation Mechanical drilling is a proven technology, but still shows a high potential for innovation. High-speed spindles, for example, exceed 250,000 rpm, and high-velocity tables enable axis speeds in excess of 2,000 IPM. Parallel processing of up to eight panels or multiple spindles per panel greatly improves the throughput of the machines and makes the process more cost effective. Higher accuracy, on the other hand, is achieved by implementing “smart” sensor technology. For mechanical drilling of blind vias and microvias, there have been different approaches to control the drilling depth. In the past, accuracy of z-axis control on the order of ⫾50 µm (⫾2 mil) could be achieved, which is not sufficient to form microvias. A breakthrough in depth control technology brought forth a new concept—the electric field sensor (EFS). The EFS generates an electromagnetic field inside of the pressure foot. The drill bit is used as an antenna to sense this field and the output signal is monitored. The monitored signal dramatically changes when the drill bit touches a metal surface, such as the copper layer of the board. The drop of the antenna signal is used to “zero” the z-axis position and drill from this reference position precisely into the board material. This way, a depth accuracy of ⫾5 µm (0.2 mil) can be expected in a manufacturing environment. Additionally, EFS is extremely robust, since it involves neither optical parts that could be disturbed by debris nor mechanical parts that could wear out. The accuracy is not even affected by surface debris. Figure 3.1 shows microvias produced utilizing EFS technology.2 EFS produces nicely shaped vias with straight-angled walls down to 100 µm (4 mil), as detailed in the images in Fig. 3.1. EFS can be used on single-spindle and multiple-spindle machines and can even be retrofitted. Therefore, EFS offers an opportunity to start manufacturing microvias using (existing) mechanical drill equipment. The importance of being able to transit from traditional drilling to microvia formation on existing equipment must not be overlooked. This allows the PCB fabricator to fine-tune upstream and downstream processes (plating, inner-layer alignment, etc.) without having to consider new process variables from the hole formation process itself. If the upstream and downstream processes are understood, faster adoption of a laser via formation tool is possible. 3.3 Comparison Among Various Via Drilling Technologies Currently, NC drilling is the most common process for generating holes in PCB. However, NC drilling is technically limited to hole sizes of 200 µm and up (not really microvias). Although smaller holes may be pos-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Mechanical Drilling
Microvias by Mechanical Drilling
127
Microvia formation with EFS depth control.
Figure 3.1
sible, these would come at the cost of significant productivity (minimal stack height). In addition, creation of blind vias is virtually impossible where typical dielectric thickness is 50 µm or less.3 In subsequent chapters, several other microvia forming technologies are introduced. Figure 3.2 shows the comparison of inner diameters for vias formed by various technologies.4 Further comparison is given in Table 3.1 as well. It is obvious that all other via-forming methods outperform conventional mechanical drilling. Figure 3.3 illustrates the via profiles with different forming processes.4 Although in general mechan-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Mechanical Drilling
128
Chapter Three
Figure 3.2 Comparison of via diameters formed by various technologies.
Figure 3.3
Typical via profiles with different forming processes.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
25–50 µm
LPI/dry film
Phototool Developer
Average (3)
Yields/cleanliness Material development
25–50 µm
Material used
Consumables
Process control
Technical challenge
Resolution
Relative rating: 1 = lowest, 5 = highest
Productivity Process development
Medium-high (2)
Dielectric cost
Low-average (4)
Phototool Photoresist Gases
Liquid/film
Low-medium (4)
(2) Coater (liquid only) Laser system (∼$500,000)
(3) Coater (LPI only) Printer Developer
Initial investment
Low (1) 2–3
High (5) 60–120
Laser drill (cladded laminate)
Productivity (panels/h)
Photovia (bare resin)
Comparison of Various SBU Technologies
Items
TABLE 3.1
50–80 µm
Cost Productivity
Average-high (2)
Phototool Photoresist Gases
Single-cladded laminates
Medium (3)
(3) Laser system (∼$500,000)
Low (1) 2–3
Laser drill (coated foil)
50–80 µm
Cost Productivity
Average-high (2)
Phototool Photoresist Gases
Coated foil
High (1)
(3) Laser system (∼$500,000)
Low (1) 2–3
Laser drill (coated foil)
75–100 µm
Cost Productivity
Average-high (2)
Phototool Photoresist Gases
Coated foil
High (1)
(3) Plasma unit ($300,000–400,000)
Low-medium (2) 12–18
Plasma etch (coated foil)
Microvias by Mechanical Drilling
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
129
Microvias by Mechanical Drilling
130
Chapter Three
ical drilling is not suitable for making microvias, compared to other processes this method has the merit of giving good via wall conditions (straight and smooth). Therefore, mechanical NC drilling is still a possible candidate for via formation in some special applications. 3.4 References 1. Lau, J. H., and C. Chang, “An Overview of Microvia Technology,” Circuit World, 26(2): 22–32, January 2000. 2. Kauf, M., L. Ekblad, and H. Martinez, “Mechanical and Laser Via Formation,” Board Authority, 2(2):61–65, July 2000. 3. Numakura, D. K., S. E. Dean, D. J. McKenney, and J. A. DiPalermo, “Micro Hole Generation Processes for HDI Flex Circuit,” Proc. HDI EXPO ’99, pp. 443–450, San Jose, CA, 1999. 4. Lau, J. H., Low Cost Flip Chip Technologies, p. 124, McGraw-Hill, New York, 2000.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Source: Microvias
Chapter
4 Microvias by Laser Drilling
4.1 Introduction Although lasers have been evaluated for use in the circuit board industry for many years, only since 1995 has laser drilling been used in mass production. As of early 1999, the total number of systems in use was estimated to be in excess of 400 units. The rate of installations is more than 50 percent greater than the previous 12-mo period, a clear indication of the rapid adoption of this technology in the organic substrate fabrication industry. This increase in the popularity of the laser as a via formation tool is due partly to the flexibility of the process and partly to the wide range of circuit board materials that are laser compatible. This provides fabricators with the lowest entry cost to high-density interconnect (HDI) available today. The rapid productivity advances provided by system manufacturers have ensured that laser technology is moving into high volume production, with more microvias formed today by laser than by any other method.1 While mechanical drilling is dominant for through-holes with large diameters, laser via formation is more favorable for blind vias and microvias. At the end of 1999, laser via formation was still limited to only a few products. Worldwide, there were 400 laser systems in production, with 300 of those systems installed in Japan. Between 2000 and 2002, this situation is expected to change dramatically. Estimates predict that 350 million phones will be needed for the cellular market in the course of these 3 years. Production of these 350 million cellular phones will require 2000 laser systems. This number does not even include the growing need for Internet communicators, personal computers, global positioning systems, and other devices.2 131
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
132
Chapter Four
4.2 Mechanism of Laser Drilling There are two mechanisms by which the laser removes dielectric materials in the drilling process. These are photothermal ablation and photochemical ablation.1 4.2.1 Photothermal ablation
As is indicated by its name, photothermal ablation is a heating and vaporization process and is generally accomplished by using a laser that operates in the visible or infrared (IR) spectrum, between 500 and 10,600 nm. The absorbed laser energy heats the material, causing it to melt and vaporize. The area around the via is affected by the heat of the process, and the via sidewall is often carbonized, requiring cleaning with an aggressive desmear process before plating. 4.2.2 Photochemical ablation
This mechanism is seen only where photo energies exceed about 2 eV, with laser wavelengths in the ultraviolet (UV) spectrum below 400 nm. These high-energy photons can break bonds at the molecular level in long-chain organic materials.3 The resulting particles, occupying more volume than their original molecules, are forcibly ejected from the via and are usually left as a powder on the substrate surface or are removed by extraction mechanisms. This process is sometimes known as a “cold” process due to the general lack of thermal damage seen around the via. The cleaning process is used optionally, and tends to be less aggressive than that required in photothermal processes. Figure 4.1a shows a via formed with the photochemical process using a UV laser, which contrasts with Fig. 4.1b, a via in the same organic material formed with the photothermal process using an IR laser.
Vias formed with (a) UV laser energy, (b) IR laser energy. Figure 4.1
(a)
(b)
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
133
4.2.3 Combination processes
In practice, the nonhomogeneous nature of printed circuit boards consisting of both organic and inorganic materials often requires that the via formation process with UV lasers be a combination of both photothermal and photochemical processes. Results indicate that UV ablation of inorganic materials (copper and glass) is a thermal process. The shallow penetration depth, high energy absorption, and short pulse of the laser contribute to a fast cutting rate with minimum collateral thermal damage to surrounding materials. 4.2.4 Absorption curves
The key to efficient laser ablation is strong absorption in the target materials at the chosen laser wavelength. Figure 4.2 shows the absorption of some commonly used printed circuit board materials.4 The absorption of resins depends very much on the additives used in their fabrication. They all absorb strongly in the ultraviolet, but have variable characteristics through the visible and infrared, where they can absorb or transmit. Copper foil is a very strong reflector down to about 60 nm, at which point its absorption increases steadily into the ultraviolet. 4.3 Types of Laser Tools for Microvias
4.3.1 CO2 laser
Most of the older installed laser systems are equipped with CO2 lasers only, working in the far IR between 9,600 and 10,600 nm. These systems use the first-generation process invented in Japan, where a CO2 laser is used for drilling of the dielectric material. The CO2 laser beam can be simply focused onto the surface of the substrate via a mask with a projection lens. A variant of the first-generation process is the CO2 ablation of unclad rigid or RigiFlex material that lends itself well to reel-to-reel applica-
Strong absorption in all materials
UV
VISIBLE
IR
Resins vary in th based on additives be almost transpa
Total Absorption
1 0.9 0.8 0.7 0.6 0.5
FR4 Matte Cu
0.4 0.3 0.2 0.1 0
Glass
Copper is refl
0.2 0.3 0.4 0.5 0.6 0.7 0.8 0.9
1 1.1 1.2
Energy absorption curves for FR-4 resin, E-Glass, and matte Cu.
Figure 4.2
Glass is transpa
Wavelength (microns)
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
134
Chapter Four
tions. A mask is imaged with a projection lens onto the surface of the material. The via diameter is then defined by the image size of the mask. Due to the long wavelength of the CO2 laser, the minimum size of the vias is also limited to approximately 100 µm (4 mil). The resulting accuracy is limited due to the tendency of unclad materials to stretch/shrink more during the lamination process than do clad materials. In addition, parallel surfaces have to be created to control impedance, and direct dielectric ablation is limited to processing only one single layer.2 To overcome some of the limitations, oxidized copper-clad material can be used to enable the absorption of the CO2 laser. The top copper layer has to be etched down to approximately 5 µm, and a black oxide layer is applied onto the surface. After the via formation process with the CO2 laser, the oxide is removed and the vias are plated. This process involves additional steps for etching, oxidizing, and later removing the oxide. Still, the attainable via diameter is limited by the long wavelength of the CO2 laser to approximately 100 µm (4 mil).2 In RF-excited CO2 laser, the gas plasma is excited by a radio frequency electrical pulse. These lasers are typically sealed units that require no external gas supplies. The rise time of the unmodified laser pulse is around 50,000 to 100,000 ns. To achieve the shorter pulses required to minimize thermal damage, some external modulation of the beam is often required. This limits maximum pulse rates to around 3000 to 4000 pulses per second.1 The transverse excited atmospheric (TEA) CO2 laser uses a highvoltage (12-kV) DC pulse to excite a gas plasma that generates a single large laser pulse. These lasers have been used in the marking industry for many years. The systems require external gas supplies, and fastflow versions of this laser can operate at between 300 and 600 pulses per second. Pulse duration varies between 100 and 1000 ns, depending on the gas mixture. Routine maintenance of these lasers involves replacing electrodes and optical components, making them more expensive to operate than the sealed CO2 units.1 The CO2 lasers have significantly higher productivity for holes larger than 70 µm in diameter. They can ablate more than 15,000 (100-µm diameter) holes through 50-µm-thick dielectric in 1 min. In general, the CO2 laser is used to drill in the dielectric layer and not to drill holes in copper, because the visible wavelength of CO2 is too large to give enough energy to penetrate the copper at high speed. Therefore, additional processing is required prior to drilling. For instance, windows must be selectively pre-etched through the copper foil at positions where holes in the dielectric are to be formed. (This is called the conformal mask method, and it presents the problem of higher costs and limitation of resolution in both vias and circuits.) Recently, Hitachi has
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
135
shown that with its CO2 laser drilling machine, it can drill through copper foil (<9 µm) by coating a layer of black oxide (called multibond in Japan) or Cobra® onto the copper. Today, the companies that supply the CO2 laser drilling machines are Hitachi, Lumonics, Panasonic (Matsushita), Mitsubishi, and Sumitomo.5 4.3.2 UV:YAG laser
The UV:YAG laser, with smaller wavelengths (255 to 365 nm) and much higher energy, is used to drill holes in the copper and dielectric (the socalled imaging method) at a much lower speed.6 UV:YAG lasers have demonstrated great capability in drilling both dielectric and copper layers, but for both processes the ablation time is proportional to the hole diameter and neither process is therefore competitive above 100-µm diameters. Thus, the YAG laser is the preferred laser for drilling when the hole diameter becomes very small—50 µm, for example. Because YAG lasers also ablate copper, it is more difficult to control the formation of blind vias using a copper stop-pad. Although the speed of the YAG is only one-tenth that of the CO2 laser, when copper is to be drilled through, some makers of high-end MLBs prefer to use the YAG because it does not require that the copper be etched to create windows. Figure 4.3 shows a cross section of a microvia made by UV:YAG laser. Today, ESI, Excellon, Exotech, Hitachi, and Sumitomo supply the UV/ Nd:YAG laser machines. Also, Hitachi and Lumonics of Canada now offer a combination of Nd:YAG/CO2 laser machines.5 4.3.3 Excimer laser
The excimer laser has a wavelength of 248 nm with KrF and 193 nm with ArF. Excimer lasers can generate holes smaller than 50 µm in diameter through dielectric or copper layers. Controlled-depth drilling is also possible, thus allowing blind vias to be created. Their slow
Figure 4.3 Cross section of microvia drilled by a UV:YAG laser.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
136
Chapter Four
drilling speed, however, makes them impractical for microvia formation. Nevertheless, the excimer laser still can drill 10,000 holes per minute through a conformal mask that has a predetermined hole pattern. However, an effective mask can only be made of quartz material and the cost of this mask is prohibitively expensive for small panel runs. Today, Litel, JPSA, and Tamarack supply excimer laser machines, to which JPSA can add either T-CO2 or diamond CO2 laser heads.5 4.3.4 Comparison among various laser tools
Table 4.1 shows the comparison between the three laser processes for microvia formation. It can be seen that there are some important benefits of using the UV:YAG lasers, as shown in the following list. ■
The capability to drill through copper, which eliminates the printing and chemical etch steps for opening windows in the outer layer
■
The capability to form microvias as small as 25 µm
■
The capability to drill multilayer vias, providing opportunities to reduce sequential buildups
Table 4.2 shows that microvias formed with the UV:YAG laser technology pass all qualification tests.7 Table 4.3 shows the test results of another case using the UV:YAG laser technology. It can be seen that the samples pass all qualification tests. This indicates that laser drilling is a robust process. That is why more than 70 percent of the world’s microvia boards are made by laser ablation. Laser-formed microvias are thermally and electrically more reliable than traditional PTHs.8 It should be noted that laser drilling of SBU PCB and substrate is still in its infancy; therefore, further research on micromachining technology and reliability engineering is necessary. In particular, the maintenance of laser pointing stability, power stability, depth of field, and system positioning tolerances are critical issues to be resolved. In addition, lasers are not very energy efficient. Thus, putting lasers into TABLE 4.1
Comparison of Various Laser Methods for Microvia Formation
Capabilities
Excimer
UV:YAG
CO2
Diameter (µm)
10–100
25–100
For copper For resin (epoxy and polyimide) For FR-4 Hole sharpness Process cost
Very slow Slow Very slow Very good High
Slow Slow Slow Good High
70–250 (50–250) No Fast Fair Slope Low
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
TABLE 4.2
137
Summary of Qualification Tests and Results Substrates tested
Results
30°C, 60% RH, 192 h, followed by three reflows at 215°C
98
Pass
MIL-STD-883 Method 1011 Condition B
500 cycles, −55°C to 125°C, liquid to liquid
98
Pass
Thermal cycle
MIL-STD-883 Method 1011 Condition B
1000 cycles, −55°C to 125°C, air to air
98
Pass
Pressure cooker
JESD22-A102-B
96 h, 15 psig, 121°C
16
Pass
High-temperature storage
MIL-STD-883 Method 1008
150°C, 1000 h
55
Pass
Temperature/ humidity/bias
JESD22-A101-A
1000 h, 85°C, 85% RH, 5-V bias
16
Pass
Test
Specification
Description
Preconditioning
JESD22-A113-A Level 3
Thermal shock
TABLE 4.3
Qualification Tests and Results
Test
Conditions
Observation
Results
Thermal cycle
−65–125°C, 30 min each 100 cycles 200 cycles 300 cycles
No corner crack Resistance <10% change
Pass
Wet proof
40°C/90–95% RH for 240 h
Resistance <10% change
Pass
Voltage
20°C/65% for 96 h and 500 V DC for 60 s
No crack of copper in the vias
Pass
Thermal shock
260°C (10 s)–25°C (20 s) for 30 cycles
No corner crack No copper lift No solder resist (S/R) lift
Pass
Solder
260°C, solder dip 10 s
No delamination No corner crack No S/R lift No delamination No corner crack No S/R lift No delamination No corner crack No S/R lift
Pass
288°C, solder float 10 s
288°C, solder float 5 s
Pass
Pass
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
138
Chapter Four
around-the-clock manufacturing tools for making microvia SBU PCB and substrate poses a great challenge.5 4.4 Material Selection 4.4.1 General considerations
There is a wide range of materials available today for microvia formation. Some of the materials known to be qualified in the PCB industry today for laser drilling are:9 ■
Allied Signal RCC® and Polyclad RCF®
■
Gore Speedboard® N and C
■
DuPont Thermount® E210, E220, and E230
■
FR-4 and FR-5 with glass fabrics: 1 × 104, 1 × 106, 1 × 1080, 1 × 1065, 1 × 2113, 1 × 3070, 2 × 104, 2 × 106, 3 × 104
■
Novaclad® Polyimide
■
Materials from other laser dielectric suppliers including BF Goodrich, Ciba, Specialty Chemical, Enthone-OMI, Hitachi Chemical, MacDermid, Mitsubishi Gas & Chemical, Park, Shipley, and Taiyo Ink.
For telecommunication applications, there are two typical resins used for microvia formation, namely, Resin Coated Copper Foil® (RCC or RCF) for subtractive PCB processes and Thermal-Curing Resin (TCR) for additive PCB processes. RCC is the material of choice for the fabrication of cellular phones. The reasons for choosing RCC and not any other dielectrics in this application are:5 ■
RCC is readily available.
■
The cost of RCC has dropped in the past few years, making it more attractive.
■
From a manufacturing perspective, it is easy to form microvias using the UV:YAG laser compared with photovia technology, and there is no need for any of the special chemical processes associated with other technologies.
■
The dielectric has a laminated thickness of 40 to 60 µm, which allows for good impedance control.
■
It is possible to make blind vias through multiple layers.
4.4.2 Laser-drillable fabrics10
One key factor of a new family of materials that enables easier laser drilling is the weaving and postweaving processes implemented by the
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
139
glass fabric suppliers. By careful formation of the glass fiber bundles, the glass manufacturer can provide a flatter bundle in both the warp and the fill directions as compared to the rounder bundles usually associated with standard E-Glass weaving technologies. Included in this new process is a spreading of the glass fibers to achieve a more even glass distribution across the entire area of the fabric. In this manner, the fabric has a smaller range of highs and lows in glass density. With standard materials, the area where two fiber bundles overlap has a high glass density and is more difficult to laser-drill. When the fibers are spread out, these high-density areas of glass fibers have a lower glass content and can be laser-machined with less laser pulses. Of course, different glass manufacturers utilize slightly different processes to achieve this spreading of fibers, but the different glass manufacturers arrive at the same resulting glass distribution characteristics. Figure 4.4 illustrates the differences between a standard EGlass fabric and a fabric that has been optimized for laser drilling. Utilizing this enhanced glass fabric and a compatible resin technology, the laminator can produce a multilayer system that has many advantages compared to resin-coated copper technology or to laminates made with conventional E-Glass fabrics. These laser-drillable fabrics are currently available in limited glass styles, but are gradually becoming commercially available in more standard glass fabric styles.11 The first materials to be utilized in the industry are presently thin fabrics, which are prepregged with high-Tg resin systems for the chip packaging applications. Although the fabric provides a building block for this technology, the resin systems utilized have to complement the glass finishes to achieve optimum performance in laser drilling.12 Table 4.4 provides the typical properties of laser-drillable multilayer materials as compared to both resin-coated copper and standard materials. As outlined in the table, fiber-reinforced materials with this
(a) Figure 4.4
(b)
Standard E-Glass fabric (a) vs. laser drillable E-Glass (b).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
140
Chapter Four
enhanced glass fabric can provide numerous advantages in the design of printed circuit boards and HDI, including improved thermal and mechanical characteristics of the finished interconnect. Another key benefit of laser-drillable fabrics is the reduction in print-through of the internal circuit pattern to the outside of the multilayer board after the pressing operation. It is not uncommon, with thin external dielectrics and thin external copper, for the pattern of Layer 2 or Layer n-1 to be transferred to the outer surfaces. This printthrough topography can reduce outer-layer circuitry formation yields when fine lines are predominant. RCC-type materials can sometimes
TABLE 4.4
Comparative Benefits of Laser-Drillable Multilayer Materials
Property
Resin coated copper
Print-through Outer dielectric tolerance Maximum laserdrillable dielectric thickness Laser-drilled hole geometry and plateability Dimensional stability Resin cracking Typical laser-drilling speed (500-Hz TEA CO2 Laser, 75-µm dielectric)* Material options (volume availability)
x-y CTE range (PPM/°C) Tg range (°C) Plasma compatibility Optimum layer counts Minimum copper (µm) BGA rework Chip packaging
30–40 130–170 Yes 2–12 5 Fair Yes
E-Glass standard materials
Laser drillable LD advanced materials
Moderate ⫾15%
Good ⫾10%
Excellent ⫾10%
80 µm
240 µm (2,3-ply)
240 µm (2,3-ply)
Good
Fair
Excellent
Moderate Possible 50 µm: 1 pulse
Good No 50 µm: 4–5 pulses
Excellent No 50 µm: 3–4 pulses
80 µm: 1 pulse*
80 µm: 6–8 pulses*
80 µm: 5–6 pulses*
Epoxy High-Tg epoxy
Epoxy High-Tg epoxy Low-loss epoxy Low-CTE epoxy APPE Polyimide Low-loss polyimide Cyanate-ester 10–16 130–250 No 2–50 5 Excellent Yes
Epoxy High-Tg epoxy Low-loss epoxy Low-CTE epoxy APPE Polyimide Low-loss polyimide Cyanate ester 10–16 130–250 No 2–50 5 Excellent Yes
* Application dependent.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
141
show more print-through than conventional materials depending on the design, the copper weight, and the lamination process. The use of laser-drillable fabrics reduces print-through because of the glass reinforcement and good surface planarity compared to standard E-Glass or resin-coated copper dielectric technologies. In addition to reduced print-through, the laser-drillable materials have inherently lower surface roughness as measured with a surface profilometer when compared with standard E-Glass dielectrics. Laser-drillable prepregs and laminates allow many options for laser microvia formation in a conventional multilayer process. Back-plane technology with high overall thickness designs can easily benefit from this approach because of the need for the lower z-axis expansion afforded by fiber reinforced dielectrics. The benefits of laser-drillable E-Glass reinforced materials include faster laser processing, cleaner hole formation, lower thermalmechanical expansion rates, better hole-wall adhesion during the metalization process, uniformity of material in the multilayer structure, easier Underwriters Laboratories (UL) approval of new products, and better fill of buried via stacks. Laser-drillable fabric technology provides other options to the fabricator and to the original equipment manufacturer (OEM) end user, including a broad spectrum of available resin systems. 4.4.3 Dielectric thickness capability and resin filling10
There are more benefits associated with laser-drillable fabric technology, namely thickness uniformity and resin filling. Most resin-coated copper technologies are somewhat limited in outer-layer dielectric thickness capability due to the process of manufacturing. Because of this limitation, certain applications of impedance control and buried via designs are more difficult to achieve. Laser-drillable prepregs and laminates offer some alternatives to enhance these types of applications. Since resin-coated coppers are relatively thin by their nature (80 µm and below), it is difficult to achieve standard impedance without external fine lines (100 µm) for microstrip applications. To complicate the issue, resin-coated coppers have slightly worse thickness tolerance compared to standard prepregs, a characteristic that does not assist in tight impedance control. This is not the case with laser-drillable fabrics, where higher overall thickness can be achieved with tighter thickness tolerance. With the thicker dielectrics provided by the laser-drillable fabrics, 50-Ω impedance can be targeted with standard external line geometries, such as 125-µm lines and spaces, thereby providing the possibility of better final interconnect yield. In addition, HDI manufacturing is often associated with buried vias, which require resin filling during the fabrication process. Usually Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
142
Chapter Four
resin-coated copper technologies have difficulty in filling buried via pairs due to the thin nature of the product. Also, with resin-coated copper, it is sometimes difficult to guarantee a minimum insulation thickness over circuit lines after the relamination. With laser-drillable (LD) fabric materials, insulation thickness of 40 µm or greater is possible, with the glass fabric acting as a spacer to guarantee the insulation between the layers. Figure 4.5 illustrates a micrograph of a cross section of a multi-layer board, which utilizes laserdrillable fabrics both internally for the buried vias and externally for the microvias. Notice the excellent filling of the buried vias by the laserdrillable prepreg. A further benefit of the laser-drillable fabric technology is its ability to be supplied as a core for buried via applications. This will enable fabricators to create vias generated by laser ablation from Layer 1 and n to Layer 3 and n − 2, respectively. This cannot be accomplished using resin-coated copper technology. Because of the glass reinforcement, dimensional stability during processing and of the final multilayer are improved with the laser-drillable fiberglass-reinforced materials compared with resin-coated copper. As shown in Table 4.4, the x-y CTE for glass-reinforced materials is considerably improved over that for resin-coated copper. A key factor in this improved x-y CTE is the low CTE of the glass fabric itself. Figure 4.6 illustrates the tighter range achieved on dimensional stability in ppm movement when utilizing the laser-drillable fabrics. 4.4.4 Laser drilling robustness10
Figure 4.7 contains two micrographs comparing the conventional 1080 dielectric to the new laser-drillable dielectric for the formation of a
Figure 4.5 Buried vias resin filling utilizing laser-drillable LD materials.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
143
Figure 4.6 Comparison of dimensional stability (106 LD and 1080 LD types vs. resin-coated foil).
microvia utilizing a CO2 laser. After four laser pulses on the dielectric, some residual resin is left at the bottom of the microvia formed in the conventional dielectric, which will disrupt the integrity of the plating process. In addition, the circumference of the resulting hole is not uniform due to the glass-rich bundles associated with conventional fabrics. On the contrary, the LD dielectric shows clean laser-drilled holes with clean lands at the bottom of the microvia. Several laser drilling equipment manufacturers now utilize multiplefrequency lasers that provide sequential processing of the laser formation of microvias. By tailoring the wavelength of one laser to remove the copper foil, the alternate laser can be made to have a different wavelength and pulse configuration that allows fast and clean removal of the glass fibers and resin, thereby forming a reliable microvia hole. These laser machines all use galvo technology for speed enhancement and provide software programming of the process to optimize the hole texture.
(a) Figure 4.7
(b)
Comparison of conventional 1080 (a) and LD (b) dielectrics (4 pulses of TEA
CO2 laser). Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
144
Chapter Four
As the technology of laser drilling and microvia processing progresses, thicker dielectric substrates, such as 1080 and 2113, become viable candidates for blind and buried via formation. With the laserdrillable prepreg and laminate materials and the new technology of dual laser drilling machines, the laser process can be adjusted to provide approximately 25 percent improvement in laser drilling speed while simultaneously providing a rounder, more plateable internal surface geometry. Since the LD fabrics do not have as many glass-rich areas, the possibility of glass wicking is reduced considerably. Although very popular, the resin types and thickness ranges of resincoated coppers are somewhat limited. For example, most resin-coated coppers have just two generic FR-4 resin categories: (1) 130 to 140°C Tg and (2) 150 to 175°C Tg. There are a few higher-performance resins that have been applied to resin-coated copper and SBU approaches. Although these products have excellent technical merit, they are not being used in high-volume nonreinforced applications at this time. The weaknesses of nonreinforced resin technology may not be readily apparent for the lower layer counts. As the layer count increases, however, a number of factors provide a compelling argument for considering fiber-reinforced options and, more importantly, laser-drillable fabrics. Higher-layer-count designs in general require lower thermal expansion in order to improve via reliability and to prevent pad lifting on the external circuitry. Also, with more complex designs, buried vias are being used more often in conjunction with blind vias to increase density. Buried vias often are designed into the HDI board as the second or third dielectric. Because of their location in the multilayer structure, they require more dimensional stability and better via-filling capability. The options for laser-drillable fabrics systems are listed in Table 4.5. Perhaps the biggest advantage of utilizing fiber-reinforced fabrics is lower CTE. 4.5 Via Formation Processes Laser drilling is a single- or multiple-via formation technology that replaces the existing mechanical drilling process. Laser drilling differs from mechanical drilling in that the focused beam used to create the vias can produce smaller holes than conventional drilling. The laser drilling process is shown in Fig. 4.8. A typical laser-drilled build-up PCB containing two blind vias and a buried via is shown in Fig. 4.9. One of the most important advantages of laser drilling is that it is compatible with many copper-clad or unclad dielectrics and reinforced or nonreinforced PCBs. Laser drilling can be used to create both blind vias and through-holes. It follows the standard multilayer process and is capable of resolving smaller features.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
TABLE 4.5
145
Advanced HDI Material Properties for LD Systems
Resin type Resin-coated copper Epoxy Epoxy Epoxy, low-CTE Epoxy, low-loss BT BT JEDEC APPE
Fiber type None HDI N4000-2 LD N4000-6 LD N4000-7 LD N4000-13 LD N5000-32 LD N5000 LD N6000 LD
Application
Tg (°C), DSC, TMA, DMA*
x-y CTE (−40 to 125°C), PPM/°C
135–140 Broad spectrum Low CTE Low CTE Low ∆k 1–5 GHz Telecom PBGA, HDI 1–10 GHz
155–170 140 180 155 210 180 190* 210*
30–40 12–16 10–14 10–14 10–14 10–14 10–14 10–14
* by DMA
4.5.1 Direct via formation
The simplest via formation method is to use a focused laser beam to directly drill the board material, including both the copper and dielectric.13 The smallest via size achievable is approximately the spot size of the focused laser beam. Larger vias can be made by expanding the laser beam optically or by moving it in a circular pattern while trepanning (Fig. 4.10) or spiraling (Fig. 4.11). The process is often used to drill
Figure 4.8 Basic process flow for microvia formation by laser.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
146
Chapter Four
A seven-layer PCB with blind-buried-blind via net.
Figure 4.9
through-holes and blind vias.14 In Fig. 4.10, the laser beam is gated on in the center of the via. It then completes a programmable number of circumferences of the via before returning to the center. This process is often used for through-hole vias with programmable diameters. In Fig. 4.11, the laser beam is gated on in the center of the via. It spirals out to the circumferences of via, removing all material to a certain depth. This process is often used for blind vias with programmable diameters. Figure 4.12 shows two 50-µm (2 mil) and one 75-µm (3 mil) vias formed by direct laser punching and trepanning, respectively. At present, only the UV:YAG laser is used for this process.
Laser Beam Trajectory
Laser Beam Turns On & Off
To Nex Via
Programmable Via Size Solid State, UV Laser
Figure 4.10 Reinforced Organic Material
Copper Plane
The trepanning pro-
cess.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
Figure 4.11
147
The spiraling pro-
cess.
4.5.2 Ablation threshold
When creating blind vias, it is important to have a drilling process that self-limits on the target conductor layer. In the case of UV:YAG laser, the fluence (or energy density) of the laser beam on the substrate is adjusted so that it is unable to ablate copper. Figure 4.13 shows the relative ablation threshold of materials used in board manufacture.15 The laser fluence is adjusted by expanding the beam diameter or attenuating the output power until it is between the values of the target dielectric material and copper. In this way, dielectrics can be removed without affecting the conductor layer (Fig. 4.14). In the case of CO2 laser, the power must be lowered to the point where copper is not vaporized, and the target conductor layer should not have a black surface that absorbs IR. 4.5.3 Multilayer vias
Most blind vias in foil constructions are formed in two steps.16 The first step removes the outer layer copper and some of the dielectric, which is used as a buffering zone. UV:YAG lasers are used almost exclusively
Direct via formation (50-µm vias formed by direct laser punching). Figure 4.12
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
148
Chapter Four
Relative Ablation Threshold 9 8 7 6 5
4.13 Relative ablation thresholds of materials used for PCB fabrication.
Figure
4 3 2 1 0 P.I./PTFE
FR4/Aramid
E-Glass
Cu
for this process. The second step removes only the dielectric, and is accomplished either with a low-fluence UV:YAG laser or a CO2 laser. The process steps are shown in Fig. 4.15; vias at each stage of production are shown in Fig. 4.16. The two steps are performed automatically in a process sequence, and require only one insertion of the circuit board into the drilling machine. The two-step process can be expanded to form vias from Layer 1 to 3 (or n to n − 2) directly (Fig. 4.17). The sequence is similar to the standard two-step process except that both conductor layers 1 and 2 are removed in the first step. The usefulness of this multilayer process is limited by present plating restrictions. Deeper vias require a proportional increase in diameter, negating some of the original benefits of microvia technology. 4.5.4 Projection mask1
In a projection mask drilling system, the image of a single via, or of a complete via pattern, is projected onto the surface of the panel to be drilled. Figure 4.18 shows the layout of a simple projection system capable of drilling a single via at a time. A hole in the mask is illuminated with the laser beam, and the image of this hole is projected onto the panel surface. The masks are typically made of material that is reflective or resistant to the laser wavelength, and the optical systems are often demagnifying, which enables a relatively low power density to be used at the mask, thus extending the mask life. In the case of lasers that have large, high-power output beams, like excimers, the mask often contains an entire via pattern and is scanned
Figure 4.14 A 75-µm via formed in resin with a UV:YAG laser.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
149
Figure 4.15 Two-step processes for laser via drilling.
by the laser beam. If a number of vias in the mask can be illuminated by the laser beam, then they can be formed at one time using larger projection optics. These masks have to be very robust and spotlessly clean; therefore, they are often made of deposited dielectric materials on quartz. Projection mask systems that form single vias require minimal tooling, but via size is dependent on the mask. If programmable via size is required, some automated way of changing the mask size must be implemented. 4.5.5 Conformal mask1
Conformal masks are generally an integral part of the panel to be processed. In the case of a printed circuit board, holes are etched in the surface copper using conventional develop-etch-strip technology. The laser beam then illuminates these holes and removes the exposed
(a)
(b)
(a) A 75-µm via in RCC after step one. (b) The rest of the dielectric is removed and the copper surface is cleaned.
Figure 4.16
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
150
Chapter Four
A 150-µm via formed from Layer 1 to 3 in two layers of RCC.
Figure 4.17
dielectric material (Fig. 4.19). This process requires the mask material either to be reflective to the laser wavelength or to have an ablation threshold much greater than that of the dielectric material; i.e., the mask material will be undamaged by the laser beam but dielectric material will be ablated. Both these situations occur in practical examples. Vias can be formed one at a time if just a single hole in the mask is illuminated. If a large laser beam is used, multiple vias can be formed at once by scanning the laser beam over the panel surface. Conformal mask via formation is very common with TEA CO2 and excimer lasers. The additional cost is attributable to the phototools required to image the via pattern on the copper surface layers of every panel and the additional develop-etch-strip processes. Via size tends to be limited by the size of the window etched in the copper, with 100 µm (4 mil) to 150 µm (6 mil) being a practical range that offers reasonable yields. Smaller via diameters can be achieved with copper-clad materials. A lithographic etching process defines the via diameter; the CO2 laser
Figure 4.18 Projection imaging— a single via is projected onto the surface of a panel.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
151
Conformal mask process—the window is etched in the copper and the dielectric material removed by laser ablation.
Figure 4.19
uses the openings in the copper surface as a mask (conformal mask) to ablate the exposed dielectric material below (see Fig. 4.20). The process uses CO2 lasers with high pulse repetition rates and high average power. State-of-the-art systems use RF-excited CO2 lasers, running in super-pulsed mode, that don’t have gas flowing through the laser and therefore don’t need any laser gas installation. After 10,000 hours or more, the laser unit is simply replaced with a refilled unit, resulting in lower cost of operation and lower downtime. RF excitation of the laser gas and super-pulsed mode ensure high peak power, a high repetition rate of up to 100 kHz, and a good beam profile close to the theoretical optimum of TEM00. This enables fast and accurate shaping of the vias. The combination of superior laser sources with high-speed and precise beam guiding and motion systems (scanners, scan lenses, and working tables) provides high-quality vias at ablation rates exceeding 60,000 vias per minute. The diameter range doesn’t depend on the laser because the copper is pre-etched, and is typically between 75 and 125 µm (3 to 5 mil). Some taper angle is preferred for easy plating of the microvia. One solution to effectively process copper-clad materials is the use of UV laser sources. UV lasers to be considered include gas lasers, such as excimer or copper vapor lasers, but their use in the PCB industry is limited due to the use of toxic gases (excimer) or long-term reliability issues (copper vapor). Broadly accepted are solid-state lasers using neodymium (Nd3+) as the laser active material. Although these are often called YAG lasers, the host crystal carrying the neodymium can
Figure 4.20
Flow chart of conformal mask process.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
152
Chapter Four
actually be yttrium-lithium-fluoride (YLF) or yttrium-vanadate (YVO). Since the laser wavelength is defined by the laser active material, not by the host crystal, all configurations share the same laser wavelength of 1,064 nm. Using laser diodes instead of lamps for pumping the laser rod results in a real all-solid-state laser. The advantage is the long lifetime of the diodes—in the range of 20,000 h instead of 500 h for arc lamps. This not only greatly reduces maintenance, but also eliminates unscheduled downtime caused by lamp breakdown. Pumping diodes have a predictable life cycle, so that replacement can be scheduled. In addition to availability and reliability, the stability of diodepumped lasers is better. Due to their broad emission spectrum, pumping lamps put a lot of heat into the laser crystal, causing thermal distortion. The consequence is lower laser beam quality and higher pulse-to-pulse fluctuations. Conversely, diodes deliver a very stable pumping light at precisely the wavelength needed for the laser process, thus avoiding undesired heat effects. As shown in Fig. 4.21, the “fundamental” wavelength of neodymium lasers can then subsequently be frequency multiplied to 532 nm (second harmonic), 355 nm (third harmonic), or 266 nm (fourth harmonic). It is important to keep in mind that in the IR the achievable resolution is low and the ablation process is of a thermal nature. This means the material is simply heated and evaporated by depositing a certain amount of energy per pulse into the bulk material. Going toward the UV range, the achievable resolution increases and the process will move toward photochemical ablation. Every photon can crack a bonding in the bulk material and thus remove the atom or molecule directly without heating effects. Photochemical ablation results in the best quality and no thermal damage to the surrounding materials.
Figure 4.21
Laser wavelength spectrum.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
153
State-of-the-art industrial UV lasers are “black-box” in design with no maintenance parts inside. After the lifetime of the diodes, the complete unit is simply replaced by a refurbished unit. There are systems using 532 nm as well as 266 nm for special applications, but the majority are working at 355 nm (frequency tripled). The minimum via diameter is defined by the diameter of the UV laser spot at the copper surface. It is possible to achieve via sizes below 10 µm (<0.5 mil), but diameters of 25 µm (1 mil) and up are common. The strategy of attaining vias with diameters larger than the UV beam spot is similar to the mechanical milling process and is called trepanning. The UV laser starts at the center of the via and moves in concentric circles with increasing diameter to ablate the copper on the complete area of the via. This shows clearly the advantage of the laser for small vias, since the processing time increases with increasing diameter of the vias. Of course, the UV laser can also be used for ablation of the via dielectric, but the ablation rate of UV light is much lower and the process has to be set up very accurately so the second copper layer is not damaged. Certain blind via drilling processes use the laser to remove the outer layer of copper. Copper’s low absorption in the infrared makes it difficult to cut with CO2 lasers without using very high power, which can cause damage to the area surrounding the via. Attempts have been made to increase the efficiency of this process by adding proprietary organic or black oxide coatings to the copper to increase its absorption. These processes are still in their infancy. 4.5.6 Dual laser via formation2
The dual-laser system is a device with both a UV and a CO2 laser. This combines the advantages of both processes: the precise and damage-free UV ablation of the copper surface and the fast and efficient ablation of the dielectric with the IR laser. Dual-laser processing is viewed as a “third-generation” process, developed independently in many different industries, mainly in the United States and Europe (see Fig. 4.22). The via size is defined by the UV laser, as described earlier, and the CO2 laser with a fixed beam diameter (up to 250 µm) is applied subsequently. Results are via sizes in the range of 25 µm (1 mil) to 250 µm (10 mil) (see Fig. 4.23). Dual-laser systems offer the broadest process compatibility. The same laser system can be used for prototype work, small batches, and large production runs. Looking at a typical PCB life cycle clearly demonstrates the advantages of the dual-laser concept; in the early design stages there are many changes in the via positions. The dual-laser process allows the fabricator to use the UV laser to define the vias in the copper and subsequently to use the CO2 laser to drill the dielectric,
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
154
Chapter Four
Figure 4.22
Flow chart of dual-laser via formation process.
avoiding high mask costs. Even the desmear process (for prototypes) can be done with subsequent UV processing (laser desmear). In a later stage, the majority of the via positions are fixed, but there are still some via position changes. Pre-etching the copper layer, the dual-laser system lets the manufacturer drill the few vias that have to be changed with the UV laser and the main part of the vias with the CO2 laser only. In a mature design with all vias well defined, only the CO2 laser is used, in combination with copper pre-etching, for highest throughput rates. An example of a dual-laser system is shown in Table 4.6. The CO2 laser is sealed, RF-excited, and super-pulsed with a maximum pulse repetition rate of 25 kHz. The UV laser is diode-pumped and Qswitched, delivering 355 nm with a maximum pulse repetition rate of 100 kHz. Fast galvanometer scanners in combination with f-theta lenses cover scan areas of 50 × 50 mm2 (approximately 2 × 2 in2) for the IR beam and 30 × 30 mm2 (1.2 × 1.2 in2) for the UV beam. Panels are handled by a vacuum chuck on an x-y table with linear motors and scales, combining a high speed of 60 m/min (2360 IPM) with a large working area of up to 610 × 711 mm2 (24 × 28 in2) and a precision of ⫾25 µm (1 mil). 4.5.7 Future trends2
Microvia formation will continue to experience frequent and rapid changes of technologies. With declining via diameter, direct dielectric
Scanning electron microscope (SEM) micrograph of a dual laser-drilled microvia.
Figure 4.23
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
TABLE 4.6
155
Dual-Laser System—LVD 2001 DP Laser generator
Laser type Wavelength Beam mode Pulse energy (max) Frequency (max) Peak power (max) Average power (max)
CO2 RF-excited, sealed off 9600 nm TEM00 1.5 mJ 25,000 Hz 350 W 80 W
Scan area (mm) Scan speed
50 × 50 1,000 pos./s, 1-mm spacing
Diode-pumped UV Q-switched 355 TEM00 0.3 mJ 100,000 Hz ∼10 kW 3.5 W
Galvonometer scanner 30 × 30 1,000 pos./s, 1-mm spacing
ablation with the CO2 laser will reach its limits. Dual-laser systems, featuring higher accuracy and the capability of processing smaller via diameters, will increase in number. To avoid the risk of investing in capital equipment that will end up as stranded assets, modular duallaser systems might be the safest investment. Dual-laser systems differ distinctly in design. Some manufacturers are bound to certain components, such as their own laser sources and scanners. Other designs are more flexible and modular, integrating components of leading brands and offering upgrades when more advanced laser sources or optics become available. Modular and flexible design enables the user to adapt the system to different processes and react to market requirements, and provides an insurance policy against obsolescence costs. Modularity doesn’t have to end with the components integrated into the system, but includes the complete design of the laser system, software, and automation capabilities. This way, the user can start with a system for manual loading and add automation components when the order volume increases. The autoloader is set beside the laser system, only occupying the left side of the machine and keeping the opportunity open to add yet another laser system to the left side of the autoloader. This way, only one autoloader per two laser units is needed, saving investment costs and floor space. Understanding the utilization factor for automation equipment dedicated to only one machine, the wisdom of feeding two machines with one automation system becomes clear. The autoloader loads, unloads, and might even flip panels, thus enabling a fully automated process starting with raw panel and ending with panels processed on both sides (Fig. 4.24). The panels are provided from the feeder cart, prealigned, and forwarded to the machine tables. After finishing side A is finished, the panels are flipped and side B is processed.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
156
Chapter Four
Figure 4.24
Material flow from autoloader to laser system.
The finished panels are then stored in the stacker cart. The concept includes drill time parallel flipping when both lasers are involved. The ideal solution depends on the product spectrum to be processed. For through-holes and blind vias with a diameter of 200 µm (8 mil) or more, mechanical drilling is surely predominant. In contrast, laser drilling is predominant for diameters of 150 µm (6 mil) and less. The gap between these technologies makes it hard for users to decide which technology to use. EFSs can clearly bridge this gap, providing an overlap down to 100 µm (4 mil) and therefore a smooth transition from mechanical to laser via formation. The via quality is excellent, and, with the opportunity to retrofit EFS, it offers an entry into microvia technology using existing equipment. This way, microvia technology can be evaluated and all production processes can be streamlined before a completely new technology is introduced. Figure 4.25 presents at the economic aspect and shows a significant increase in costs when drill diameters of 150 µm (6 mil) or 100 µm (4 mil) are used. The higher costs are caused by a higher tool (drill bit) price and a reduced via formation (hit) rate. Combining these two costs results in significantly higher cost per via for diameters of 150 µm (6 mil) and 100 µm (4 mil), while the costs per via for diameters of 200 µm (8 mil) and larger are nearly constant. The laser becomes more favorable with smaller via sizes. Applying the dual-laser formation, the ablation of the copper with the UV laser is the limiting time factor. The area to be ablated is scaled to the square diameter of the via. The economic crossover point is approximately 150 µm (6 mil), where dual-laser drilling becomes more economical than mechanical drilling. Conformal mask processing with CO2 laser involves the highest investments in wet chemical processes and lithographic equipment,
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
Figure 4.25
157
Comparison of via drilling costs.
but has the lowest running costs per via due to the extremely high drill rates achieved. It is therefore the process of choice for high-volume production (assuming that the board fabricator already has an investment in clean room resources for photolithographic processes). As with any manufacturing decision, there are other factors to consider that drive the process selection. Besides the issue of obsolescence risk, one needs to consider the supply chain, particularly if there are plans to export the processes abroad. Prior to moving PCB fabrication overseas, one must ensure that equipment providers have sufficient support infrastructure to provide parts, training, and assistance. Finally, there may be specific process needs that are required by a particular PCB fabricator (automation, laser wavelengths, beam path, etc.) that will push equipment providers into semi-customization of their equipment. 4.6 Practical Laser Drilling Systems1 4.6.1 Parallel projection imaging systems
Laser drills that project images of multiple vias or entire circuits are very similar to optical imaging systems (Fig. 4.26). The laser beam is scanned over a projection mask that is imaged on the surface of the panel. These systems are rarely used in the fabrication of printed cir-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
158
Chapter Four
Figure 4.26 Simplified diagram of a projection mask system.
cuit boards, but have had extensive use in multichip module and package manufacturing. 4.6.2 Sequential via formation systems
These machines make up the vast majority of systems in use today by the PCB industry. The beam positioner is the most critical subsystem in the laser drill. It has a number of important functions: ■
To focus or project the laser spot with equal size and power density over the entire drilling area
■
To place the laser beam accurately in the drilling area
■
To move the laser beam at very high speed between drilling locations, or within drilling locations if trepanning and spiraling techniques are used
The two most common beam positioning systems available today are the galvanometer with x-y table combination and compound beam positioner. 4.6.3 Galvanometers with X-Y tables
The deflection galvanometer has become a very common tool in laser beam positioning over the past 30 years. Figure 4.27 shows a simplified galvanometer beam positioner layout. Very small rotations of the mirrors deflect the laser beam over a relatively large area. These systems are very fast, with random positioning times of between 1 and 4 ms.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
Figure 4.27
159
A simplified layout of an x-y galvanometer system.
In practice, galvanometer systems have a number of limitations: ■
In an uncorrected state, they project the laser at an angle to the work surface. This is unacceptable for most via drilling, so special telecentric lenses have been developed to keep the beam orthogonal to the work surface, no matter at what angle it enters the lens system (Fig. 4.28).
■
In drilling applications, they are usable only over small areas, typically 50 mm2 (2 in2) or less; and their accuracy degrades exponentially toward the edge of the field.
To solve the accuracy problem, galvanometer systems are used in conjunction with x-y tables. The galvanometer drills a small section of the field, and then the table steps to the next position. In this way, the
A telecentric lens keeps the laser beam perpendicular to the work piece at all times.
Figure 4.28
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
160
Chapter Four
A compound beam positioner. The galvanometer and linear motors all move continuously during the drilling process.
Figure 4.29
panel is drilled as a series of small squares that are butted together to cover the entire area. Care must be taken to avoid abutment errors in these systems. At the join between two squares, the positioning error between two adjacent vias is the sum of the total positioning error of the x-y table and the galvanometer system. These abutment areas should be kept away from high-density via arrays. 4.6.4 Compound beam positioners
This technique uses a combination of cross-axis linear motor and galvanometer technologies to create a system that can effectively drill with multiple laser pulses on the fly (Fig. 4.29). The linear motors and galvanometer systems are moving continuously during the drilling operation. When a via is being drilled, the laser beam is held in position over the correct location by counteracting motions of the linear motors and galvanometers. Fast motions between vias are accomplished by the galvanometers alone. There is no stepping between areas covered by the galvanometer, as the movement between vias is continuous, thus avoiding abutment errors. The future for laser drilling looks bright. Every year sees advances in laser sources, beam positioning technology, and compatible materials. There is every reason to assume that productivity will continue to double on an annual basis, making this technology a difficult one for alternative via formation methods to catch. 4.7 References 1. Cable, A., “Microvia Generation Equipment—Laser,” Board Authority, 1(2):40–46, June 1999. 2. Kauf, M., L. Ekblad, and H. Martinez, “Mechanical and Laser Via Formation,” Board Authority, 2(2):61–65, July 2000. 3. Brannon, J., “Excimer Laser Ablation & Etching,” American Vacuum Society Monograph, 1993. 4. Owen, M., H. Bleiweiss, J. V. Puymbroeck, E. Roelants and A. Mattelin, “The Introduction of UV YAG Laser Drilled Microvias in PCBs,” Proceedings of PC World Conference, 1996. Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Microvias by Laser Drilling
161
5. Lau, J. H., and C. Chang, “An Overview of Microvia Technology,” Circuit World, 26(2):22–32, January 2000. 6. Cable, A., “Microvia Formation in Flip-Chip Packages Using a New Diode-Pumped Ultraviolet Laser Technology,” Proceedings of SEMICON, Singapore, 1999. 7. Petefish, W. G., D. B. Noddin, and D. A. Hanson, “High Density Organic Flip Chip Package Substrate Technology,” Proceedings of the 48th ECTC, pp. 1089–1097, Seattle, WA, May 1998. 8. Young, T., and F. Polakovic, “Thermal Reliability of Laser Ablated Microvias and Standard Through-hole Technologies,” Proceedings of the IPC Expo, p. S17–2, Long Beach, CA, March 1999. 9. Raman, S., J. H. Jeong, S. J. Kim, B. Sun, and K. Park, “Laser (UV) Microvia Application in Cellular Technology,” Proceedings of the IPC Expo, p. S17–6, Long Beach, CA, March 1999. 10. Forcier, B., “Laser Drillable E-Glass Multilayer Materials: An Overview of Laser Enhanced Materials,” Board Authority, 2(2):67–70, July 2000. 11. Forcier, B., and F. Hickman, “The Design and Fabrication of HDI Interconnects Utilizing Total Integration of Fiber Reinforced Materials,” Board Authority, 2(1):64–68, April 2000. 12. Kimura, Y., “Specially Developed Glass Fabrics for Ultimate Small Diameter Hole of High Density Package Board by Build-up Method,” Proceedings of IPC Expo, April 2, 2000. 13. “Ultraviolet Laser System and Method for Forming Vias in Multi-Layered Targets,” U.S. Patent 5,593,606, January 14, 1997. 14. Noddin, D. B., P. Fischer, W. L. Gore, and E. Swenson, “Solid State UV-Laser Technology for the Manufacture of High Performance Organic Modules,” Proceedings of 48th ECTC, May 1998. 15. Cable, A., “New Laser Processes and Wavelengths for Drilling Through-Hole and Blind Vias in a Wide Range of Circuit Board Materials,” Proceedings of IPC Printed Circuits Expo, San Jose, CA, 1996. 16. “Method Employing UV Laser Pulses of Varied Energy Density to Form Depthwise Self-Limiting Blind Vias in Multilayered Targets,” U.S. Patent 5,841,099, November 24, 1998.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Laser Drilling
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Source: Microvias
Chapter
5 Microvias by Photoimaging
5.1 Introduction The first commercially used PID was a modified liquid solder mask produced in 1990 by IBM at Yasu, Japan. Modern PIDs are in the form of either liquid or dry film. For photovias with liquid photodielectric, the dielectric is curtain-coated and cured, microvias are exposed, and the dielectric is developed. Then the panel plating follows with patterning to create signal traces. For photovias with dry-film photodielectric, the dielectric is laminated, microvias are exposed, and the dielectric is developed. Panel plating follows with patterning to create signal traces.1 There are many PID materials available in the market, such as Probelec by Ciba, ViaLux PDDF by DuPont, ENVISION® PDD-9015 by Enthone-Omi, and photoimageable resins produced by Dow, MacDermid, Morton, Shipley, Taiyo Ink, etc. The determining factors in materials selection depend upon the characteristics required. These can be categorized by dielectric type, e.g., epoxy or polyimide; the form the dielectric takes, e.g., liquid or film; and general physical characteristics of the dielectric, such as Tg, dielectric constant, or moisture absorption. In selecting a dielectric material on the basis of these criteria, both manufacturing choices and end product design requirements must be taken into consideration.2 5.2 Photoimageable Dielectrics for Microvias 5.2.1 Typical process for photo-defined vias2
Microvias can be formed in mass production by photoimaging technology. The dielectric is applied over the base substrate, and the microvias are 163
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
164
Chapter Five
imaged and developed. Then this via layer is cured, adhesion-promoted, and copper-plated to connect the microvias. A final primary resist is applied to complete the outer-layer imaging; then the circuits are etched or pattern-plated. Conductive paste can also be used to fill the microvias and circuit pattern. A step-by-step process flow is illustrated in Fig. 5.1. ■
Step 1. The photosensitive polymer is applied to the base substrate.
■
Step 2. The coated substrate is exposed to UV light through a rightreading mask containing the desired circuit pattern to selectively cross-link the material.
Figure 5.1 Process flow chart for fabricating multilayer PCB using photoimageable dielectric and conductive ink technology.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
165
■
Step 3. The dielectric is developed, removing the un-cross-linked polymer, leaving the final photoexposed, cross-linked polymer with the desired conductor pattern.
■
Step 4. The conductive ink is applied to fill the photoexposed conductor holes.
■
Step 5. A second layer of photosensitive dielectric is applied and exposed to a mask containing the pattern of the vias.
■
Step 6. Step 3 is repeated.
■
Step 7. Step 4 is repeated. The vias are filled with conductive ink and cured.
■
Step 8. A third layer of photosensitive dielectric is applied. This layer is then exposed, developed, filled, and cured with the circuitry for the second conductor layer. Figure 5.2 shows a cross section of a photo-defined via.
5.2.2 Liquid photoresist systems3
There are a growing number of liquid photoresists being developed for the PCB and photochemical milling (PCM) industries. Within this array of products, a variety of different photochemical systems are used that impart unique properties to the finished photoresist materials. Factors such as resolution, photospeed, and chemical resistance are affected by the choice of these systems. Several of these liquid photoresist materials are reviewed and compared here, along with the process and application techniques for their use. All of these photoresist systems rely on exposure to light to create differential solubility between the exposed and unexposed regions. A negative-working resist relies on exposure to photopolymerize or cross-link the material to produce a region that is insoluble in a developer solution. Positive-working sys-
Figure 5.2
Cross section of photo-defined microvia.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
166
Chapter Five
Figure 5.3
Solubility in a devel-
oper.
tems create regions of enhanced solubility in a developer in regions where the resist is exposed. The difference between the soluble and insoluble regions of the material can be thought of as the resist contrast (see Fig. 5.3). 5.2.2.1 Negative free-radical resists. A negative-working free-radical system uses a photoinitiator that, upon exposure to light, creates free radicals. These free radicals initiate a chain reaction with the monomers, causing them to polymerize and hence harden the photoexposed areas. This hardening prevents the developer solution from solubilizing the exposed area. The sensitivity of the system to various wavelengths of light (spectral sensitivity), which affects photospeed, can be tuned through the use of a sensitizer. The sensitizer will absorb light at a wavelength usually different from the photoinitiator and then act as an energy transfer agent to aid in the formation of additional reactive free radicals. The sensitizer can then return to its ground state and participate in further reactions. Additional exposure will continue the cross-linking reaction. The more cross-linked the system becomes, the more resistant the material is to developer solutions (see Fig. 5.4). 5.2.2.2 Negative cationic resists. A variation of the negative-working cross-linking scheme is found in the negative cationic system. Here the
Figure 5.4
Negative free-radical
reaction.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
167
cross-linking occurs through the aid of an acid catalyst. The photosensitive material is a photoacid generator (PAG). Upon exposure to light, the PAG forms an acid, which is mobile in the resist matrix. When heated, this acid catalyzes a reaction between reactive sites on the polymer chains with reactive sites on the cross-linker (a novolac polymer and a melamine cross-linker are shown in the example in Fig. 5.5). The extent of the reaction that occurs depends on the amount of acid generated, the amount of heat applied, and the length of heating time. The example in Fig. 5.5 shows up to six reactions occurring per crosslinker molecule. 5.2.2.3 Positive diazonaphthoquinone (DNQ) resists. The common positive-working system is based on a photoactive compound (PAC) and soluble binder reaction, which has been a mainstay of the microelectronics industry for chip manufacturing. This system typically starts with a novolac binder, which by itself has solubility in base (OH−). To this binder is added a PAC that lowers the solubility of the entire mixture. The PAC is a DNQ. When exposed to UV light, the DNQ forms a ketene intermediate that, in the presence of water, forms an indene carboxylic acid (see Fig. 5.6). This acid species enhances the solubility in base of the
Figure 5.5
Negative cationic reaction.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
168
Chapter Five
Figure 5.6
DNQ photolysis. Figure 5.7
DNQ-novolac solubility.
entire resist system to a level much higher than that of the PAC-novolac mixture or the novolac binder alone (see Fig. 5.7). 5.2.2.4 Positive cationic resists. Another version of the positiveworking system utilizes the cationic deblocking reaction, sometimes referred to as chemical amplification. This system was developed to address the photospeed problems encountered in deep-UV (DUV) exposure and is now beginning to see widespread use in the semiconductor industry. The energy outputs of most exposure systems at DUV wavelengths are small compared to the mid- and near-UV. To combat this deficiency, these systems use a PAG to create the acid catalyst for the reaction. In this case, the reaction is a deblocking of a dissolution inhibitor from the backbone polymer (see Fig. 5.8). This acid catalyst reaction improves the photosensitivity of the material by orders of magnitude. Also, the choice of dissolution inhibitor will affect the initial solubility of the photoresist and change the resulting solubility contrast, usually improving it over the level achieved with PACnovolac resists (see Fig. 5.9). So far, these resists have not been applied in the chemical milling or PCB industries.
Figure 5.8
Positive cationic reaction.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
Figure 5.9
169
Photoresist solubility.
5.2.3 Direct-write film4
Laser direct imaging (LDI) offers one solution for elimination of steps. Direct imaging is a gigantic leap in the PCB manufacturing process. LDI eliminates the entire phototooling area and puts imaging directly into the chemical process of the PCB manufacturing. This is a radical change in the entire manufacturing process and requires tight control and process monitoring. Not every company is ready or able to commit the resources required to make this leap. Direct-write film or film that is imaged thermally also offers a way to eliminate steps and to simplify the entire process of phototool production without drastic changes to the current manufacturing process. It offers an alternative to the major change required when laser direct imaging is introduced into the process. Phototools must provide a clear and sharp circuit image with quality that satisfies fabricator requirements for imaging onto photoresists. Silver halide film imaged on a photoplotter is a proven technology for providing phototools. This technology has been in use since 1964, when the first photoplotter was invented. These early photoplotters used a vector technology to move a beam of light across silver halide film to produce the circuit image. This process was slow and not very flexible but got the job done. There have been many improvements in photoplotters over the years. Photoplotters today use lasers in a raster format to produce high-quality tools in minutes instead of hours. The raster plotters can create very complex images out of the arrays of laser dots. Circuit boards today are much more complex, with smaller features and tighter tolerances. Raster laser photoplotters have provided fabricators with the means to generate phototools that can accommodate today’s geometry requirements. There have also been major improvements in silver halide films. However, the basic process is the same. First the film must be acclimated to the temperature and humidity in the photo area. After being exposed to light, the film goes to an automatic processor for developing. The processor includes a developing solution tank, a fixer tank, a water Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
170
Chapter Five
rinse tank, and a dryer section. The film is subject to extreme humidity and temperature changes that cause it to change size. The film must then go through a stabilizing time to restore the correct image size before it can be used in production. There are then two alternatives regarding how to use the film. The film may become the master copy, and contacting it to diazo makes a working phototool. As the diazo deteriorates due to use, more diazo can be contacted. The other method is to use the original as the working phototool and create new original masters off the photoplotter as needed. The first-generation phototool provides the best-quality image because it is the original. Newer silver halide films offer improved resolution and sensitivity that allows them to produce the higher-quality images required for today’s complex technology. Silver halide film, however, still requires time to acclimate and time to stabilize after being subjected to heat and moisture in the processor. This stabilization time is becoming a bigger factor as production cycles decrease and costs increase. Environmental restrictions have put pressure on PCB fabricators regarding the handling and disposal of the chemicals and waste associated with silver halide. These factors all contribute to the need for direct-write film. Direct-write film produces phototools without the need for chemical processing. These films are thermally imaged using high-powered lasers that use the laser energy to alter the media and create dark areas and light areas. Several direct-write films have appeared on the market over the years, including ones from AGFA, Kodak, and Polaroid. Mastertool from AGFA is one of the direct-write films that has created a lot of excitement in the industry. It eliminates the need for chemical processing and the associated stabilization time. Because it has no gelatins, there is no need for acclimation before exposure. It is very dimensionally stable. Mastertool consists of a polyester base with a layer of bismuth on the base. A thin polyester sheet is laminated on top of the bismuth to protect the material. A high-powered laser melts the bismuth, which then solidifies into extremely fine drops. These drops are sufficiently dispersed to permit light to pass through the media. Unfortunately, the method has a problem. The drops remain in the media and result in the Dmin being significantly higher than for silver halide film. Special attention and care has to be used in the contacting process. Care has to be taken in setting up the exposures using Mastertool film. More light is required—and for a longer time. Mastertool is not a direct replacement for silver halide in the contacting process, and this has hindered the wide acceptance of Mastertool in PCB applications. Ideally, a film must fit right into the current process without the need for special setups. Still, because of the advantages of directwrite film, there are a large number of Mastertool users.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
171
The interest generated by Mastertool does show the need in the industry for this type of solution. Mastertool and other direct-write films are still offered in the market. More films will continue to appear on the market to fill the need in the industry. Key to their success will be the convenience of use and quality of image. The film must be daylight-safe, with no need for a darkroom. Ideally it should allow direct digital exposure (no over- or underexposure due to processing), it must have no wet processing (no waiting for stabilization, no chemicals, and no processor maintenance), and it has to be translucent for easy registration (no need to contact to diazo). The film must have a low UV Dmin and a high UV Dmax so it can be inserted into the existing process with a minimum of changes to the process. It should be used like silver halide film yet still eliminate the steps users are looking to shed. A film with these characteristics will serve a broad spectrum of the market. Fast-turnaround shops will appreciate the elimination of the processing and stabilization time. Medium- and long-run fabricators will benefit from the resistance to scratching and film deterioration. All users will appreciate the elimination of chemical processing and the associated environmental concerns. The basic price of the direct-write film does not need to compete directly with the price of silver halide film. Users will still recognize costs savings. These savings will come from eliminating the darkroom, the costs of processors and chemicals, and the need to make diazo and waste material processing—along with the labor associated with these steps. Recently a new type of direct-write film has been under development. This direct-write film shows promise of filling industry needs. The film has been chemically formulated to be imaged on the Barco Prism IR imager that has an internal drum architecture. An internal drum consists of a stationary concave surface. A vacuum holds the medium to the inside surface of the drum. Above the drum, a rotating mirror scans the laser across the drum while the entire optical assembly moves continuously down the drum. The internal drum platen allows the medium to remain stationary, thereby making it easier to accommodate many types of flexible media. The laser is an Nd:YAG infrared laser that transmits large amounts of energy to the medium to create an image. The construction of the film is shown in Fig. 5.10. The key to the technology is the IR-absorbing layer. This IR layer bonds the dye coat to the polyester base and is totally environmentally friendly. The dye coat is also bonded to the top coat, or what is called the peel layer. When the laser (Fig. 5.11) ablates the IR-absorbing layer, the dye coat is no longer bonded to the base. The top layer (peel coat) remains bonded to the dye layer. In Fig. 5.12, the peel coat has been removed, and that portion of the dye coat that is no longer bonded to the base is removed with the peel coat. The
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
172
Chapter Five
Figure 5.10
Direct-write film (before Figure 5.11
exposure).
Direct-write film (after
exposure).
bond of the dye to the IR layer is stronger than the bond to the peel layer, so the unablated material and dye remain on the film base. The peel coat may be disposed of easily without special environmental care. This finished film looks very much like diazo but has been imaged like film. It is used just like silver halide film, except that it is daylight safe, is direct-digital exposed, and involves no wet processing. The film is translucent for easy registration and has a low UV Dmin, a high UV Dmax, and an infinite shelf life. It appears to satisfy all the criteria users have for direct-write film. 5.3 Surface Laminar Circuit Technology5 5.3.1 Configurations and design rules
Surface Laminar Circuit (SLC) technology was the first of the microvia build-up technologies to reach the interconnect market in volume. Development of SLC technology began during the late 1980s at IBM’s development laboratory in Yasu, Japan, and the first product was introduced in 1990. The first flip chip direct chip attach product employing SLC technology was shipped from Yasu in 1992, and in 1995 IBM shipped the first printed wiring boards that utilized SLC technology from the company’s Endicott, New York, site.6 SLC technology was originally conceived as an alternative to multilayer lamination as a way to make multilayer PCBs. Instead of cir-
Figure 5.12
Direct-write film (after
peeling).
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
173
cuitizing several double-sided cores and subsequently laminating them to make a multilayer PCB, SLC technology builds up each signal layer on top of the previous layers in a sequential fashion. The base under all of the outer build-up layer is a conventional double-sided circuit board containing voltage and ground planes. All signal interconnections between layers are made with photo-defined microvias. Mechanically drilled and plated holes are used only to make connections to the backside of the laminate base and to accommodate mounting pinned components. As SLC technology evolved, its usefulness was significantly enhanced with the build-up layers on a multilayer subcomposite. This allowed design and fabrication options, such as striplines for controlled impedance, using the higher-density, more expensive build-up layers for component escape wiring while employing less dense, lowercost multilayer PCB technology for component interconnect (global wiring). It is advantageous from a wiring density standpoint to use PTHs, which extend only through the base PCB structure and not through the build-up layers, especially when two or more build-up layers are used. These internal interconnects are termed resin-filled PTHs (RFPs). RFPs allow designers to use the board area above the RFP holes and lands for wiring on the build-up layers, significantly improving wiring density. Fig. 5.13 shows a partial cross-section with three SLC technology build-up layers on one side of a multiplayer base PCB with RFPs.7 The photoimageable solder mask [photoimageable dielectric/(PID)] materials were chosen as interlayer dielectrics due to their proven compatibility with the PCB assembly process and their ability to withstand exposure to service environments, as well as having the necessary via imaging characteristics. SLC technology was originally developed and implemented with a liquid photoimageable solder mask applied by curtain coating. In 1995 it was also qualified with a dry-film
Figure 5.13 Cross section of a typical SLC 3+3 structure with filled PTHs and a staircase of microvias going from the PTH to the upper surface.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
174
Chapter Five
TABLE 5.1
Design Rules of SLC Technology Feature Size (µm) Feature
Standard
High-density
Prototype
Future
Photovia diameter (min) Photovia land diameter, top/bot (min) Line width (min) Space (min) Line thickness (min) Dielectric thickness (min) Stacked photovias
125 300 75 125 18 40 No
100 200 50 75 12 30 No
70 110 30 40 7 30 No
50 80/70 20 30 5 20 Yes
photoimageable dielectric. The liquid and dry-film PIDs have virtually identical electrical properties, and have been qualified using the same accelerated stress tests and acceptance criteria.8 Current design rules for SLC technology build-up layers are given in Table 5.1. Larger PCBs can be designed with more relaxed rules to achieve optimized yields and minimize the cost.9 5.3.2 SLC processes10
SLC technology is based on the use of photoimageable polymeric systems to form blind microvias in the dielectric material between layers of circuitry. The use of PIDs allows all microvias on a panel to be formed in parallel, with no incremental per-via cost. Its use is particularly advantageous on applications having high densities of vias (e.g., more than 50,000 on an 18 × 24-in. panel). Figure 5.14 is a typical flowchart of the SLC technology fabrication process, including the options for multiple build-up layers and RFPs. Figures 5.15 and 5.16 provide a pictorial representation of the required processes. At this level the process for SLC technology is the same whether a liquid or dry film PID is used. Figure 5.17 presents flowcharts that include details for the PID processing, highlighting the process differences between liquid and dry-film PIDs. The liquid and dry-film PIDs do give slightly different via wall profiles. The liquid PID has tapered via walls, as seen in Fig. 5.13, while the dry-film PID has essentially vertical via walls, as shown in Fig. 5.18. The tapered via walls provide good plating coverage on the via walls and base; the vertical walls allow for a smaller via top opening, and correspondingly smaller capture land, for a given via bottom diameter. The use of a liquid PID requires two unique pieces of equipment: a curtain or slot coater (with associated drying ovens) and a leveling tool (surface sander). Curtain coaters are common tools in many PCB shops, but if a shop does not already have one, installation of a curtain
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
175
Circuitize Inner Layer Cores Filled Sub-Composite PTH Option
Laminate Sub-Composite No Sub-Composite PTH Option
Drill, Plate, and Fill Sub-Composite Holes
Apply Photoresist, Expose, Develop, Etch, and Strip Last Build-Up Layer Only
Apply, Image, and Cure PID Layers 1 to N-1
Drill Composite Holes
Surface Treat for Cu Adhesion Plate Vias and Surface
Repeat N Times
Apply Photoresist, Expose, Develop, Etch, and Strip After Last Build-Up Layer
Apply Solder Mask and Surface Finish Profile Cards from Panel Final Test and Inspect
Figure 5.14
Process flow chart for SLC technology.
coater to produce SLC technology PCBs represents a significant capital investment (several million dollars). The leveling tool is required to planarize the surface of the cured liquid PID to accommodate fine-line photolithography on its surface. The liquid PID provides a conformal coating over the underlying circuit features, producing nonuniform planarity. The leveling operation also removes a lip of exposed PID that overhangs the via openings in these processes.
(Case of 1 double sided build up layer) Base Core (with circuitized layers)
Drill Thru Hole
Circuitize
Cu Plate
Apply Dielectric
Photo Via Build
Figure 5.15
Circuitize
Solder Precoat
Schematic diagram of SLC process flow.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
176
Chapter Five
(Case of 1 double sided build up RFP) Base Cores (with circuitized layers)
Apply Dielectric
Drill Thru Hole
Photo Via Build
Cu Plate
Cu Plate
Resin fill
Circuitize
Schematic diagram of SLC process flow with resinfilled PTHs.
Figure 5.16 Circuitize
Solder Precoat
Liquid PID
Coat & Dry Liquid PID (1st side)
Dry Film PID
Vacuum Laminate (2 sides)
Expose & Develop PID (1st side)
Pre-Bake PID
Partial Cure PID (1st side)
Expose PID (2 sides)
Coat & Dry Liquid PID (2nd side)
Post Expose Bake PID
Expose & Develop PID (2nd side)
Develop PID
Full Cure PID (both sides)
UV Flood and Cure PID
PID process details for SLC technology.
Figure 5.17
Level PID Surfaces
Inspect & Repair (optional) PID
Inspect & Repair (optional) PID
Cross section of an SLC microvia with dry-film PID.
Figure 5.18
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
177
The use of a dry-film PID requires only one unique piece of equipment: a vacuum laminator. Vacuum laminators are common in the production of PCB; in addition, the capital to obtain one is significantly less than that required for a curtain or slot coater. The dry-film PID has excellent planarization and does not require a leveling process due to the film’s low solvent content and low shrinkage and the vacuum lamination process. 5.3.3 Reliability and applications
Normal reliability requirements for SLC technology PCBs include the following tests (zero fails): 1. Temperature/humidity/bias ■ 85°C/85 percent RH/5 V, 1000 h ■ 110°C/85 percent RH/5 V, 150 h 2. Thermal cycle ■ −40 to 65°C, 5 cycles ■ −25 to 115°C, 2500 cycles 3. Flammability ■ UL 94 V-0 SLC technology products may also be qualified to meet additional requirements for specific applications. SLC technology has been used to manufacture high-density PCBs for integrated circuit package substrates, computer and communications equipment, and consumer electronics. Board sizes up to 65 in2 (400 cm2) have been produced in high volumes. Figure 5.19 is an example of the system board used in one of IBM’s ThinkPad laptop computers, and Fig. 5.20 illustrates the main board used in a Sony digital camcorder. Figure 5.21 shows a high-end 3-D graphics adapter having four layers
Figure 5.19 ThinkPad motherboard with SLC technology.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
178
Chapter Five
Figure 5.20 Sony digital camcorder motherboard with SLC technology.
3-D graphics adapter card with SLC technology.
Figure 5.21
of build-up on each side, and Figs. 5.22 and 5.23 illustrate single- and multichip IC modules used on this graphics card. Many of the SLC technology products have been used with chip scale packages and direct chip attach, both flip chip and wire bond. 5.4 Laser Direct Imaging11 High-density interconnection positions a spectrum of technologies and processes on the PCB fabricator’s capability roadmap. The printed circuit board industry is continually moving toward smaller features to achieve the interconnect density required by present and future packaging technologies. As feature sizes decrease and signal speeds increase, the demands on the manufacturing processes for low defect density and high quality become increasingly stringent. Accordingly, the lithography of HDI circuits—namely the patterning of conductors and pads—becomes a most demanding stage in the fabrication process. Substantial efforts have been directed at meeting HDI fabrication challenges by continuous improvement of various process stages. However, lithography requirements seem to have been neglected. LDI systems naturally lend themselves to addressing these HDI challenges. In addition to their proven advantages in obviating phototooling and Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
179
Flip chip single-chip module with SLC technology.
Figure 5.22
Flip chip multichip module with SLC technology.
Figure 5.23
repeated defects in a standard fabrication environment, they provide an indispensable tool for HDI fine-feature requirements. Laser direct imaging in general and thermal direct imaging in particular provide a readily available patterning tool for high-density interconnection fabrication. The ultrafine feature imaging capability matches or exceeds the most demanding HDI pattering applications. The precise patterning capability offered by thermal direct imaging (TDI) may, in some cases, become an enabling capability for HDI PCB manufacturers; higher density and more complex parts can be accepted for production, thus enabling fabricators to shift a higher percentage of their production capacity to higher-density and highermargin jobs. In addition to fine-line patterning capability, LDI lends itself readily to microvia formation. It utilizes “best-fit” registration of the imaged pattern to the drilled microvia holes on each individual panel through real-time hole location recognition and adaptation. Positive liquid resist provides good coating for via holes, eliminating the need for land area associated with dry-resist tenting, actually enabling padless via holes. LDI also may be used for CO2 laser drilling conformal mask generation. It is also a high-capability patterning tool for demanding Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
180
Chapter Five
controlled-impedance applications. The combination of accurate hole generation and image registration, which eliminates the need for land, is expected to influence future design rules.12–15 5.4.1 HDI lithography capability
HDI involves a variety of applications, materials, and processes. The following capabilities are directly or indirectly related to lithography: ■
Finer lines and spaces. These are most commonly 3 mil and under. Packaging substrates utilize 2-mil lines and spaces as mainstream. Figure 5.24 illustrates how routability options on the mounting layer become scarce with increasing IC complexity and higher I/O count. Clearly, fine-line imaging capability, down to 2 mils or less, would allow for more interconnections per layer, thus decreasing interconnect structure by lowering the layer count. In the extreme case, shown in the lower left corner of Fig. 5.24, only an imaging capability of 2-mil lines and spaces enables production of an interconnect structure for this IC type.
■
Smaller holes. With HDI technology, 50-µm via holes become commonplace. Made possible with the advent of laser drilling, smaller holes are being drilled to increase circuit board density.
■
Smaller pads. With smaller via holes, smaller pads are possible. As illustrated in Fig. 5.24, small pads allow for more tracks per channel on HDI circuit boards.
■
Tighter registration. Feature-to-feature, pad-to-hole, and side-to-side registration all require higher registration accuracy of smaller features and tighter spaces between them.
Figure 5.24
Routability options with high-I/O ICs.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
■
181
Tighter line width control. This control is necessary for impedance uniformity and for buried resistors and capacitors.
LDI has proven itself as a viable patterning tool for demanding applications. Most currently available systems use UV light on UVsensitive resist for imaging. These LDI machines generally work with a special LDI dry-film resist that is four to five times more sensitive than the standard UV dry film in order to provide an acceptable productivity level. A recently introduced TDI system works with an IR light source on a matching liquid resist (thermal resist). This system’s strongest feature is its extraordinarily sharp and consistent imaging capability. Some of the benefits discussed in this section are unique to the TDI system, and are accordingly pointed out. With the high-definition patterning capability of thermal direct imaging, HDI application limits are pushed further. Fine-line capability down to 2-mil lines and spaces becomes common practice with TDI. High-resolution patterning coupled with thin liquid resist facilitates improved fine-line capability. This combination allows the use of existing wet process lines commonly used in conventional intermediate interconnect fabrication processes. The following thermal direct imaging characteristics provide key advantages for HDI lithography. First, high-definition direct imaging with 5-µm resolution is achievable, along with a 5-µm square spot for sharp and accurate feature definition. A thermal positive resist with binary reaction provides true digital-quality imaging with a wide process latitude. With a positive etch resist, levels of near-shorts and microshorts are significantly reduced or eliminated. The positive-working liquid resist is suitable for tent-and-etch microvia processing. The tent-and-etch process, also known as the panel plating process, allows a straightforward sequence with a lower number of process steps when compared to a pattern plating process. The use of liquid resist allows coating thickness down to 5 µm, which provides higher-accuracy imaging and etching at a lower cost, as well as reduced material waste. Also, TDI allows the elimination of film-based defects, costs, and processing time while enabling work flow flexibility of direct CAM-to-panel imaging. A higher etch factor, characteristic of thin resists, enables narrower spaces, avoiding microshorts and near-shorts associated with lower etch factors. 5.4.2 Subtractive patterning
Features—including conductors, spaces, and pads—are getting smaller for ordinary applications, and even smaller for HDI applications. Boards with 2-mil lines and spaces along with 2- or 3-mil annular rings are not uncommon.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
182
Chapter Five
Subtractive processing is highly regarded as a straightforward printand-etch process, very similar to the inner-layer patterning process. Positive liquid resist, which protects via holes, makes this process feasible. Furthermore, hole wall protection capability may be the only factor that allows small annular ring capability in a panel-plating process. In fact, positive liquid resist may even allow padless hole patterning. Figure 5.25 is a demonstration of a padless feature generated by thermal direct imaging technology. This imaging capability naturally fits in a build-up process utilizing laser drilling over an RCC layer. In such cases, the subtractive microvia process is inherently adequate. The patterning process would be tentand-etch. Tenting the vias with dry resist poses a growing difficulty as annular ring sizes shrink. As the annular ring becomes smaller, the dry tenting patch has less hold area, which in turn gives rise to a likely via failure. Positive-liquid-resist-based LDI—with its via wall protection capability—makes patterning of such features possible. 5.4.3 LDI as conformal mask for laser drilling
CO2 laser drilling involves the formation of a mask that defines the location and extent of the vias to be drilled. With RCC material, the mask is the copper, which cannot be drilled by a CO2 laser. Thus, the mask preparation here involves the standard print-and-etch process of the microvia holes to be drilled. Thermal direct imaging aids CO2 laser drilling with its high definition and high geometric accuracy. The holes defined by a TDI system are very accurate and feature a controlled diameter. In addition, hole location is very precise due to the inherent geometric accuracy of the system. 5.4.4 Controlled impedance lithography
High-speed applications (i.e., mobile communications) require tighter impedance control. Controlled impedance impacts lithography in the
Figure 5.25 Micrograph of a 75-µm via in a 50-µm trace.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
183
following two areas: line width control and interlayer registration. Line width uniformity requirements as tight as 2 percent have been presented to fabricators for applications requiring controlled impedance. Such tight line width control capability is rare in conventional PCB lithography systems due to their inherently loose edge definition. Thermal direct imaging addresses this demanding requirement by providing a sharp edge and precise line width control. TDI process capabilities that meet or exceed these requirements have been demonstrated with unmodified wet-processing equipment. Another aspect of controlled impedance is the registration between pads or conductors on the opposing sides of a panel. This is also significant in high-frequency applications such as mobile communication devices. The issue becomes particularly critical with HDI technologies, where the dielectric material is considerably thinner compared to standard applications. LDI offers the capability of precisely registering to existing holes, ensuring resultant pad-to-pad registration. 5.4.5 Registration capability and accuracy
As HDI pushes the envelope of circuit density, it also increases the requirement for much tighter registration. With much smaller laserdrilled via holes, smaller pads around such holes are designed to enable more tracks per channel. This in turn calls for drastic improvement of pad-to-hole registration, leading to smaller annular rings. Since LDI obviates the dimensional instability of phototools, substrate feature placement is inherently more accurate. The ability to accurately locate pads facilitates the smaller tolerance of pad location relative to the holes; hence, the pads can be made smaller, saving precious board real estate. Moreover, as a real-time imaging system, LDI can adapt imaging to varying board dimensions. By looking at existing features on the board during imaging time, the system can adjust geometric parameters to best fit the microvias and other board features. This further enables smaller pad or annular ring size and further saves space to be used for denser routing. Film-based imaging uses artwork having preset dimensions, which cannot be modified unless a new film is plotted with different dimensions. While exposure machines align the films to targets on both sides of the panel, this alignment merely rotates and shifts the x and y axes of a fixed image to its panel. Minimization of image-to-target misalignment is usually achieved by optimizing (dividing) the errors among all the targets used. With exposure machines, no scaling correction can be applied to the image in order to fit the misplaced targets. A feedback procedure may be used after stripping, in which the scale of the image may be modified to fit the observed distortion of the postimaging process. This is done by producing a new film with the optimized corrected scales. Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
184
Chapter Five
Laser direct imaging has inherent capabilities for improved image registration. The circuit image is given as a CAM bitmap file that can be modified before or during the actual imaging process, as opposed to a film “hard copy” that is fixed for all panels imaged with that film. Through manipulation of the image data and the LDI electronics, the image can be manipulated to compensate for misplacement errors, thus improving imaging registration. Such modifications may be universal (global scale or rotation) or local (compensating for nonlinear errors). Figure 5.26 shows a few examples of image data manipulation that LDI can implement as part of registration compensation. The image scale can be modified locally by controlling position-dependent variations in the laser exposure (pixel) rate or by altering the relative speed between the imaging head and the panel. Figure 5.26a illustrates this for one axis, while Fig. 5.26b shows a combined effect of changing a linear scale in both axes. For example, scale
Figure 5.26
LDI image adaptation.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
185
reduction in the y-axis can be achieved by gradually increasing the pixel imaging rate in the y-axis while the imaging operation progresses in the x-axis, and maintaining a constant relative speed between the laser beam and the substrate. Alternatively, the relative speed in the y-axis between the laser beam and the substrate may be gradually reduced, while the pixel imaging rate remains constant. Such a method can also be used locally to compensate for nonlinear hole misplacement. Another example focuses on controlling the start timing of the actual scanning. This facilitates a local shift profile, such as the one shown in Fig. 5.26c, in which the start position in the y-axis changes while the x-axis speed is constant. This results in local corrections in the y-axis.
5.5 Special Considerations and Reliability 5.5.1 Notes on photo-defined vias2
The benefit of using photo-defined via technology is that it can form thousands of vias at once (i.e., it is a mass production process). However, there still are several drawbacks to the use of photo-defined via technology that should be noted. ■
Only photosensitive dielectric can be used, instead of the wide range of dielectrics that can be used with laser drilling technology.
■
Making a dielectric photosensitive can degrade its electrical performance and reliability.
■
Photovia technology is limited to blind vias with small aspect ratios (less than 2:1); vias must be formed and plated at every layer.
■
This approach cannot be used with laminated metal foils.
■
Minimum via size in production is limited to about 75 µm with most technologies.
■
This technology generally requires starting with a rigid PCB core and building outward; this core has generally poor flatness (nonuniform dielectric thickness) and dimensional performance.
■
Photovias cannot go through unpatterned metal layers.
5.5.2 Design guidelines and equipment with photo-defined vias
Table 5.2 illustrates some design guidelines for dry-film or liquid-type photosensitive dielectrics. Via diameter can be as small as 50 µm and trace width can be less than 25 µm. In comparison, via diameter can be 25 µm for laser drilling.16 The equipment needed for photo-defined via technology includes exposure unit, developer, and wet processor. The suppliers of exposure units Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
186
Chapter Five
TABLE 5.2
Comparison of Dry-Film and Liquid Types of Photoimaging Technology Dry-film type Epoxy acrylic
Applicator
(Vacuum) laminator
Thickness range (µm) Minimum opening (µm) Trace width Electrical performance Chemical resistance Handling Cost
Liquid type
Polyimide
Epoxy
Polyimide
25–50
Roll laminator Screen print Spray coat Curtain coat 25–50 10–25
Screen print Spray coat Roll coat 10–20
70
70
70
50
50 Good
50 Good
50 Good
25 Excellent
Acceptable Easy Fair
Good Difficult High
Good Fair Low
Very good Difficult High
are Bacher, Byers, Colight, Csun, Dupont, Dynachem, Gyrex, Hi-Tech, Mirmir, Morton, Olec, Optical Radiation, ORC, Peak Measuring, Tamarac, and Theimer. The suppliers of developer are Advanced Chemill Systems, ASI, Chemcut, Ciba-Geigy, Circuit Services, Danippon Screen, Glenbrook, James River, Lantronic, Microplate, Quantum, Rexham Graphics, and Technifax. The suppliers of wet processors (develop-etchstrip) are ASI, Chemcut, Hollmuller, Lantronic, and Schmid.2 5.5.3 Reliability data
Some qualification tests reported in the literature17–19 show promising results for photo-defined via technology. Also, photovia processes are currently being used. Ibiden, IBM at Yasu, and Micro Via, Inc. are already running volume production. 5.6 Impact of HDI on Fine-Line Lithography20 With pin densities increasing above 20 I/O per cm2, and total pin counts for high-end devices quickly exceeding 300 pins, area-array technology has become the interconnect package technology of choice. While 1-mm BGA pitch is standard for high-end applications today, 0.8- and 0.5-mm pitch are also in limited use, and will become more predominant as predicted by the National Technology Roadmap for Semiconductors. These fine-pitch packages, which include ball grid arrays and chip scale and flip chip packages, will all require interconnect lines and spaces that are predicted to reach 10 µm. While microvia and other build-up technologies have proven their ability to meet the exacting requirements of fine-line interconnects, patterning solutions have only recently made significant improvements. Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
187
Contact printing processes are rapidly approaching maturity and will have great difficulty supplying the patterning needs for costeffective fine-line production. LDI solutions have the ability to record fine features and provide best-fit image registration, both pivotal in breaking through fine-line patterning roadblocks. LDI is presently being introduced in high-performance PCB production environments. As this technology becomes accepted, PCB and high-density interconnect suppliers will gain flexibility and quality improvements. The concept of “each board is an original” (typified by laser printing processes) can create new opportunities for custom and semicustom applications. 5.6.1 Current technology limitations
To provide the technical solutions in a cost-effective manner, development needs to take place within the existing PCB manufacturing process. Conventional technology is limited for three major reasons. First, the conventional drilling processes limit feature sizes to about 100 µm with 50-µm placement accuracy. Second, the inherent instability of organic material creates extreme registration errors as a result of processing. Third, the abilities of conventional imaging systems to produce dense features with good yields are reaching their limits. A partial solution to the drilling problem is through the use of microvia, or build-up multilayer processes. As shown in Fig. 5.27, the first inner layers are processed conventionally, with conventional vias. A thin layer of laminate is applied with heat, pressure, and vacuum to fill the conventional holes. The copper is then etched down to 3 to 5 µm, allowing microvias to be laser-drilled or photo-etched. Copper is then redeposited to about 20 µm, covering the board and contacting the outside copper contact pads of the conventionally processed core. The plate is then laminated with dry-film resist and the board returned to finish
Figure
5.27
Typical
microvia
construction.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
188
Chapter Five
with conventional processes. A completed example of this process is shown in Fig. 5.28, which is a cross section taken from a BGA package carrier (interposer) in a Fujitsu cellular phone. Examination of the conventional blind vias displays the processing-induced registration errors. These registration errors can be significant, and are induced during the lamination process. Each layer that consists of an epoxy-fiberglass core will distort under the pressure (up to 200 psi) and heat (up to 350°F) of lamination. This distortion can vary with direction, and may be nonuniform as well. Circuit board material such as FR-4 can change by as much as 4 to 6 µm/in., and other organics such as polyimide can change by 25 to 50 µm/in. The registration problem can be solved one of two ways: use of materials with very low coefficient of thermal expansion (CTE) to minimize shear stresses, or compensation for the movement. While discussion of the first solution is outside the scope of this paper, the second solution is at the heart of it. Conventional imaging systems for PCB and high-density interconnect (HDI) are traditional contact printers, one-to-one projection scanners or, more recently, step-and-repeat projection printers. All three have advantages and disadvantages, depending on the size and type of features to be imaged. Contact printers are well known to the PCB industry and are low in cost and have low recurring tooling cost and good productivity for many applications. However, these tools have no ability to scale the artwork to compensate for distortion, and will not match the feature size and overlay accuracy required by HDI and microvia technology. (Some fabricators have achieved marginal success with feature size by reducing the field to less than 14 × 14 in2, but the distortion and scaling compensation issues remain.) One-to-one projection scanners have much better resolution capability than contact printers, are known solutions, and can image over large substrate sizes. The phototool is typically glass and thus has higher recurring costs. Again, these systems suffer from poor overlay accuracy and do not provide scaling compensation for the laminate distortions.
Eight-layer photovia multichip package carrier on six-layer main board.
Figure 5.28
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
189
Step-and-repeat systems have made a brief appearance, and can meet the resolution and overlay requirements for HDI. They are also able to compensate for scaling to some extent, but cannot independently scale orthogonal directions. The image size is limited to 4 × 4 in2, which relegates this tool exclusively to interposer imaging; it cannot be used for general PCB applications. Glass masters again make the recurring tooling costs expensive. 5.6.2 Market drivers
Evolution of technology within the semiconductor industry has continued to drive interconnect densities to higher levels, requiring more sophisticated packaging solutions. As the pin counts increase above 20 I/O per cm2, area-array technology has become the predominant packaging solution. This can be seen from the Semiconductor Industry Association (SIA) roadmap (Figure 5.29), where high-end packages quickly exceed 1000 pins. Quad-flat packs are predicted to have maximum pin counts of about 300. With the majority of product categories exceeding this pin count within the next several years, area-array technology will dominate package and interconnect solutions. While pin count is increasing, the spacing between contact points must decrease. An example of this is seen in the high-end ASIC devices, pin counts of which are predicted to be around 5000 by the year 2015. If the spacing of ball grid arrays remains at around 1 mm, then the interposer (carrier) will need to be at least 3 in. per side to sustain this number of pins! The National Technology Roadmap for Semiconductors (NTRS) (Fig. 5.30) displays these trends more clearly. Ball grid array, chip-scale packaging and flip chip substrates all require higher-density package solutions. Within 5 years, the infrastructure to support 0.65mm array pitch should be in place. This technology will require feature sizes that will extend down to 10 µm.
SIA package pin count segmented by product category.
Figure 5.29
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
190
Chapter Five
First Year of IC Production
1997
1999
2001
2003
2006
2009
2012
BGA SUBSTRATES PTH pitch (mm) 1.0 0.8 0.65 0.50
FINE PITCH BGA/CSP Line width/spacing (µm) 50 / 65 40 / 50 30 / 35 25 / 33
FLIP CHIP SUBSTRATES Line width/spacing (µm) 50 / 50 34 / 38 30 / 30 20 / 20 10 / 11 Research Required
Development Underway
Qualification/Pre-Production
This legend indicates the time during which research, development, and qualification/pre-production should be taking place for the solution.
Figure 5.30 NTRS interconnect roadmap—ball pitch and line width/spacing targets. (Source: National Technology Roadmap for Semiconductors)
Not only is pin count increasing, but the cost per cm2 of board area is decreasing, and the total number of array packages is predicted to exponentially increase as through-hole processes are replaced. Pin grid, ball grid, and chip-scale packages all display this enormous growth potential, as seen in Fig. 5.31. 5.6.3 LDI benefits and challenges
LDI tools are more complex than conventional tools, and have demonstrated the ability to record fine-line features. LDI provides other
Comparison of organic substrate market price.
Figure 5.31
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
191
important features that are pivotal in breaking through the roadblocks to large-area HDI patterning. The tool must accommodate the processinduced panel distortions, meet production throughput requirements, and maintain sufficient process latitude to support the subsequent development and etch processes. LDI tools are unique in that each image can be considered an “original.” This implies that each image can be customizable to accommodate some specific process artifact. This customization can range from bar coding of each image within a panel to specification of unique image “compensation” values, which change the image database to precompensate for a priori distortions. At current technology feature sizes (greater than 50 µm), linear image scaling that is independent for the x- and y-axes of the image is sufficient. As the feature sizes and accuracy requirements decrease, higher-order distortions may come into play. This could mean that generalized image mapping and nonlinear “predistortion” might be required to accommodate the instability of the media. LDI tools differ significantly from conventional phototools in that they replace production tools that perform massive parallel processing (e.g., contact printing of the entire image) with the serial process of rasterimaging a bitmap. As feature sizes decrease, the amount of information to be processed increases. (Note: with conventional imaging, the serial bitmap imaging process still exists, but it takes place offline, where the time to image does not significantly impact the production throughput.) In addition, the resolving power of the imaging system increases. 5.6.4 Future tool requirements
To compare existing to future LDI tool requirements, we can borrow a concept from the field of information processing known as spacebandwidth product (SBP): SBP = (number of pixels) × (average data rate) This metric is a measure of the amount of information handled within a given period. However, this metric alone does not adequately describe the complexity of the imaging system, since the pixel size could be arbitrary. Since the f-number of the optical system is proportional to the pixel size, and since SBP is an area function, we can divide the SBP by ( f-number)2 to give a more useful comparative metric. Figure 5.32 shows a potential LDI roadmap, including two additional raster-imaging tools for comparative purposes. At the low end is a conventional drum laser photoplotter. At the high end is a mask pattern generator used for fabrication of IC photomasks. As resolution of the
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
192
Chapter Five
Potential LDI roadmap compared to conventional photoplotter and semiconductor mask pattern generator.
Figure 5.32
LDI tools increases, so does the information content and the complexity of the optical systems. Two inferences can be made from this rough comparison. One could conclude that given current technology, the cost of the 10-µm-feature LDI tools would start to approach that of IC mask pattern generators. A second inference could be made that a revolutionary change to the technology base is required to provide cost-effective solutions. Clearly, reduction in the metric SBP/( f-number)2 will yield a less costly solution for a given performance level. Reduction in the amount of information to be handled by the LDI tool is one way to manage the space-bandwidth product issue. One technique is to minimize the number of pixels required to image a minimum feature size. This leads to an artifact of LDI systems known as grid snapping, as shown in Fig. 5.33. Here, the image bitmap is shown for a 4-pixel per minimum line width data set. Grid snapping to the nearest pixel location is evident, especially on diagonal lines. This artifact can be minimized by increasing the number of pixels per minimum feature. However, for a given maximum average data rate, the throughput of the tool will be reduced by the increased number of pixels in the bitmap.
Bitmap of 4-pixelper-minimum-feature database displaying grid snap artifacts.
Figure 5.33
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
Microvias by Photoimaging
193
Theoretical aerial image of a 25-µm feature (6.25-µm pixels with 6.25-µm spots). Figure 5.34
Another method to manage the SBP/( f-number)2 metric is to reduce the optical resolution. For example, a 25-µm feature can be imaged using four 6.25-µm laser spots on 6.25-µm grid (pixel) spacing, or it can be imaged using four 12.5-µm laser spots on 6.25-µm grid spacing. While the 12.5-µm laser spot system could potentially be more cost effective, there is a significant reduction in process latitude. This is evident in the computer simulations shown in Fig. 5.34, which illustrates that the 12.5-µm spots give shallower aerial image sidewalls than the 6.25-µm spots for a 4-pixel-per-feature image. The larger spot size will require better control over the resist chemistry, process, and exposure to retain equivalent control in feature resolution and critical dimension parameters. As the semiconductor industry creates components with greater pin counts and higher pin densities, the interconnect industry must keep up with higher-resolution tools and processes. While development of the LDI tool faces definite technical challenges ahead, the ability to meet the expected roadmap targets will also be dependent upon photoresist suppliers, material manufacturers, and process developers. As feature sizes continue to shrink, even the cleanliness of the process environment must continue to improve. The ability of the PCB and HDI industries to provide a solution will not be dependent upon any one technology. Communication and cooperation between suppliers will continue to be pivotal in achieving success. 5.7 References 1. Estes, W. E., T. R. Overcash, S. Padlewski, B. D. Neve, E. B. Murray, R. E. Anderson, R. C. Mason, J. P. Lonneville, W. L. Hamilton, and M. Periyasamy, “Photodielectric Dry Films for Ultra High Density Packaging,” Proceedings of SMI, pp. 47–53, San Jose, CA, September 1997. 2. Lau, J. H., and C. Chang, “An Overview of Microvia Technology,” Circuit World, 26(2):22–32, January 2000.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Photoimaging
194
Chapter Five
3. Sutter, T. C., “Liquid Photoresist Systems—An Overview,” Board Authority, 1(3):22–29, October 1999. 4. Manas, J., “Direct Write Film,” Board Authority, 1(3):14–17, October 1999. 5. Barr, D., and D. O. Powell, “Technology from Japan: Surface Laminar Circuit (SLC) Technology,” Board Authority, 2(1):87–90, April 2000. 6. Tsukada, Y., “Surface Laminar Circuit and Flip Chip Attach Packaging,” Proceedings of 42nd ECTC Conference, 1992. 7. Tsukada, Y., S. Tsuchida, and Y. Mashimoto, “Surface Laminar Circuit Packaging,” Proceedings of 42nd ECTC Conference, pp. 22–27, 1992. 8. Boyko, C., F. Bucek, V. Marovich, and D. Mayo, “Film Redistribution Layer Technology,” Proceedings of 2nd International MCM Conference, pp. 196–199, 1993. 9. Carpenter, R., and I. Memis, “SLC: An Organic Packaging Solution for the Year 2000,” Proceedings of NEPCON-West Conference, 1996. 10. Tummala, R., E. Rymazewski, and A. Klopfenstein, Microelectronics Packaging Handbook, Subsystem Packaging, Chapman & Hall, pp. 265–268, 1997. 11. Atiya, Y., “Thermal LDI: Meeting HDI Lithography Challenges,” Board Authority, 2(2):10–14, July 2000. 12. Ganjei, J., “Advantages and Disadvantages of Liquid vs. Dry Film,” Printed Circuit Fabrication, May 1997. 13. Ehlin, M. J., “The Wonderful World of Laser Direct Imaging and How to Realize It,” Board Authority, 1(3):50–55, October 1999. 14. Atiya, Y., and E. Halevi, “An Innovative LDI,” CircuiTree, June 1998. 15. Taff, I., and H. Benron, “Liquid Photoresist for Thermal Laser Direct Imaging,” Board Authority, 1(3):66–71, October 1999. 16. Numakura, D. K., S. E. Dean, D. J. McKenny, and J. A. DiPalermo, “Micro Hole Generation Processes for HDI Flex Circuit,” Proceedings of the HDI Expo, pp. 443–450, San Jose, CA, September 1999. 17. Gonzalez, C. G., R. W. Wessel, and S. A. Padlewski, “Epoxy-based Aqueous Processable Photo Dielectric Dry Film and Conductive Viaplug for PCB Build-up and IC Packaging,” IEEE Trans. Adv. Packaging, 22(3):385–390, August 1999. 18. McDermott, B. J., and S. Tryzbiak, “The Practical Application of Photo-defined Microvia Technology,” Proceedings of SMI, pp. 199–207, San Jose, CA, September 1999. 19. Nargi-Toth, K., and P. Gandhi, “Manufacturing Methodologies for High Density Interconnect Structures,” Proceedings of the CSI Technical Symposium, pp. 63–70, San Jose, CA, September 1998. 20. Tamkin, J. M., “The Impact of HDI on Fine-line Lithography,” Board Authority, 1(3):56–59, October 1999.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Source: Microvias
Chapter
6 Microvias by Etching
6.1 Introduction The development of very complex ICs with extremely high I/O counts and steadily increasing clock rates has forced electronics manufacturers to develop new packaging and assembly techniques. In addition, more and more electronic devices have to be portable and, consequently, system integration, volume, and weight are rapidly gaining importance. At the same time, the pressure to eliminate any environmental impact and to reduce cost is exponentially increasing. As a result of these considerations, the future substrates have to be hightech, low-cost interconnects characterized by very fine lines and spaces and the use of microvias, as both through-vias and blind vias as well as combinations thereof. In addition, the increasing demand for 3D packaging calls for flexible and rigid-flexible designs and highlights the importance of new interconnect substrate technologies able to cope with these recent and emerging requirements in modern electronics.1 Microvias can be formed by various etching techniques. Plasma etching and chemical etching can be extremely cost effective for generating high volumes of small holes in dielectric layers. In either case, the process cost is derived from the number of holes in a given working area. The basic principle of via etching is to create a mask that defines the positions and sizes of the holes. This may be achieved by using dry film to image, then etching a hole pattern in a copper layer, or simply by using the dry film as the etch mask by imaging and developing. Both methods are isotropic such that they etch inward while they etch downward. All holes are generated simultaneously, and the process time is dependent on how long it takes to erode or dissolve the unmasked dielectric. Plasma etching has the added benefit of removing 195
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
196
Chapter Six
organic contaminants, and with careful conditioning the amount of slope (undercut) created in the hole can be minimized. Both plasma and chemical etching processes can create blind vias, usually using the target pad as a means of defining the bottom of a blind via.2 6.2 Etching Processes 6.2.1 Chemical etching
Chemical etching is the least expensive process for generating small holes on dielectrics. Wet etching by hot KOH has been used for polyimide films. This formation technique is capable of mass via generation in that all vias are formed at the same time without regard to number or diameter.2 6.2.2 Plasma etching
The dry etching process requires procedures such as plasma etching and copper thinning (etch-back). Microvia hole (MVH) formation by gasmicrowave plasma (GMP) has been promoted by Dyconex of Switzerland and its licensee, Hewlett-Packard. Dyconex has 16 licensees worldwide because it sells a basic plasma drill for $55,000, compared to a laser drill that costs $500,000 and up or a photoimaging facility that requires around $300,000. The plasma equipment can be obtained from Advanced Plasma Systems, Inc. or Plasma Etch Inc. A step-by-step process flow is illustrated in the following list: Step 1. Fabricate core by standard double-sided rigid or multilayer board methods. Step 2. Laminate adhesive-coated copper foil to core. Step 3. Print and develop via pattern. Step 4. Etch via pattern and strip etch resist. Step 5. Plasma-ablate dielectric and etch copper overhang. Step 6. Electroless-copper-plate panel. Step 7. Laminate photo resist; print and develop outer-layer image. Step 8. Pattern-electroplate copper. Step 9. Strip resist and etch. There are some plasma-etchable materials like adhesiveless polyimide foil, FR-4 buttered Cu-foil, Aramid-paper-reinforced FR-X, liquid crystal polymer (LCP), and Cu foil buttered with FR-5 or polyimide glass or cyanate ester (CE) resin.2
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
Microvias by Etching
197
6.3 Plasma Etching for Via Formation 6.3.1 Plasma ablation3–5
Plasma has long been known as a dry-etching medium and is widely used in the semiconductor industry for the formation of very fine features. In 1991 Dyconex (Zurich) started to apply plasma ablation for the mass formation of microvias in organic material.2 Since then, the technology and the related equipment have been developed for volume production of rigid, rigid-flexible, and flexible HDIs and multichip modules (MCMs) for almost any kind of applications. The process is known as DYCOstrate®. The basic process sequence is shown in Fig. 6.1 for through-vias as well as blind vias. Usually, the base material is a copper-clad dielectric where the copper is in a first process used as an etching mask for the plasma ablation. In order to generate the mask, the copper is photochemically patterned by conventional PCB technology (via definition). When thin dielectrics, such as polyimide films, are used, the plasma generates micro-through-vias (Fig. 6.1a), whereas blind microvias are formed when a target pad is placed underneath the opening in the copper mask (Fig. 6.1b). In the case of through-vias, the overhanging copper fringes generated during the isotropic plasma etching process are too small and do not affect the subsequent plating. When blind vias are etched, the copper overhang can be critical and, due to shielding effects and a reduced exchange of chemicals, reliable plating is not possible. Therefore, a proprietary hole-forming method has been developed. During this process, the copper fringes are etched off completely and, at the same time, the total thickness of the copper layer is reduced to approximately 5 µm. This process allows the blind microvias to be plated without any addi-
Process flow chart for plasma-etched through-hole and blind vias.
Figure 6.1
(a)
(b)
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
198
Chapter Six
tional precautions and, additionally, minimizes the overall copper thickness, resulting in an improved yield in the subsequent photochemical patterning of the outer layers. Figure 6.2 shows microsections of a through-via with a diameter of 60 µm and a blind microvia with a diameter of 100 µm. As is clearly visible in Fig. 6.2b, the thickness of the plated copper is very uniform, a result of the teacup-shaped microvia. Another important advantage of plasma drilling is that it is a parallel process: all via holes are formed simultaneously. In order to maximize throughput and optimize etching uniformity, dedicated plasma drilling equipment has been developed that allows the simultaneous front and back processing of six panels (18 × 24 in2). In addition to the formation of microvias, plasma can also be used as a micromilling tool to form any kind of microfeatures. Figure 6.3 shows a summary of various possibilities that have all been applied already in specific applications. 6.3.2 Build-up constructions
The use of microvias automatically implies so-called sequential build-up constructions, as in the ceramic multilayer technology. In general, there are basically two build-up options, depending on the dielectric material used. For flexible dielectric materials, in many cases a rigidizing carrier is necessary in order to stiffen the flexible substrates locally or completely.3 In the case of rigid dielectric materials, a rigidizer is not necessary, yet with the drawback of being restricted to rigid applications only. The whole concept of this technology approach is shown in Fig. 6.4.
Polyimide
(a)
(b)
Micrographs of plasma-etched (a) through-hole via and (b) blind via.
Figure
6.2
Various microstructures processable by plasma ablation.
Figure 6.3
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
Microvias by Etching
199
Basic concept for plasmaprocessed HDI substrates.
Figure 6.4
In addition to the two options, combinations of flexible and rigid build-ups can be designed for specific requirements. Figure 6.5 shows a number of microsections taken from various examples used in medical devices, avionics, telecom, etc. While some of the build-ups are very simple, others are extremely complex, particularly when constraining cores with CIC, CMC, or carbon fibers are used. The nomenclature 3D2C3D, for instance, means that there is a three-layer DYCOstrate® on the backside. One particular build-up has turned out to be very powerful and at the same time cost effective. This build-up is a 4D construction, as shown in Fig. 6.6. Besides all the pros regarding the electrical performance, like EMI shielding, less cross talk and improved signal integrity, the total thickness of this build-up is approximately 200 µm. When such a substrate is bonded to a heat sink, the thermal management is improved substantially—in particular when thermal microvias are placed underneath the hot ICs. Although only two signal layers are available for routing, the achievable wiring density is extremely high due to via-pad diameters of 200 to 250 µm and lines and spaces down to 50 µm. Such a 4D construction can often be substituted for a 16-layer conventional multilayer board, and has been successfully used for complex, high-end MCM applications.
Figure 6.5 Selection of build-up constructions with plasmaetched microvias.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
200
Chapter Six
Advantages of a standard 4D build-up.
Figure 6.6
6.3.3 Special considerations2
Even though plasma technology can form many vias at one time, there are several drawbacks, as shown in the following list, that limit popular acceptance of plasma techniques. ■
Plasma batch processes are suitable only for small volumes or prototypes.
■
Plasma techniques usually have a via size limit of 75 µm.
■
Isotropic etching results in undercutting (anisotropic etching is desired.)
■
Plasma techniques require removal of the copper-clad overhang from blind via holes prior to copper plating.
■
Plasma techniques rely on a special resin-coated copper foil (nonreinforced dielectric layer).
Figure 6.7 shows a via generated by the plasma etching process. Compared to the microvias created by laser drilling (Fig. 4.3) and photoimaging (Fig. 5.2), the via formed by plasma etching shows undercut. This is why the plasma etching process cannot surpass the laser drilling and the photoimaging processes.6,7
Figure 6.7 Cross section of plasma-etched microvias.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
Microvias by Etching
201
6.4 Applications of Plasma-Etched HDI Plasma processing, well known in the semiconductor industry, can also be applied very successfully in the production of flexible and rigidflexible substrates. The possibility of ablating not only microvias, but also profiles, windows, etc., in a very cost-effective way, opens up totally new opportunities for the design and production of high-end, low-cost HDI and MCMs. The concept of combining a thin and flexible highdensity interconnect substrate with almost any kind of support carrier also allows optimization of the overall performance of a substrate in terms of thermal management, CTE matching, and/or mechanical rigidity. The technology, known as DYCOstrate®, is very reliable and approved for all demanding applications, from automotive uses and implantables to extreme space applications.1 6.4.1 Flexible HDI 6.4.1.1 Hearing aids. The 2D substrate shown in Fig. 6.8 has a total length of approximately 56 mm and is used in a high-end hearing aid device. The design is very innovative and the circuit contains various plasma-milled features: ■
Plasma-drilled microvias 60 µm in diameter
■
Plasma-milled large holes and windows
■
Plasma-milled profile
■
Plasma-milled blind microholes
The circuit has several assembly areas that are connected by integrated flexis. The assembly areas are surrounded by a small sealing rim, in which a row of small blind holes is etched (Fig. 6.9). A microsection through one of these blind holes is also shown in Fig. 6.9. It clearly shows that the depth of the hole is just about half the total dielectric thickness and the undercut is present with this holeforming process. The reason for this micromechanical feature is to provide a mechanical anchoring for the injection mold material applied after assembly. The mold is pressed into the cavities and hardened. As
Figure 6.8 Two-dimensional flexible HDI for a high-end hearing aid.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
202
Chapter Six
6.9 Sealing rim with plasma-etched microfeatures.
Figure
a result of this, the foil cannot be peeled off the mold, and the reliability of the final assembly is substantially increased. Forty pieces of this particular circuit on one manufacturing panel and 12 panels simultaneously processed in the plasma drilling equipment result in 480 pieces drilled, profiled, and milled in about 15 min. 6.4.1.2
Sensors. Figure 6.10 shows a two-layer flexible DYCOstrate®
(2D) with several microfeatures manufactured by plasma milling. The circuit is assembled on one side only and is folded together like a little box in order to minimize the volume. The fold lines are partially perforated by plasma. The backside is used for shielding and for the placement of some test pads. In addition to the microvias as well as some larger via holes, plasma is use to mill the profile and the perforation in the fold lines and to ablate windows and alignment holes. Also, a cable fixture is included in the outline. All these features are etched in one single process. 6.4.2 Rigidized flexible HDI 6.4.2.1 Pacemakers. Figure 6.11 shows the traditional way of making a ceramic-based substrate for an implantable pacemaker. Usually, the substrate is manufactured in 4 × 4-in2 or 5 × 5-in2 ceramic panels,
Foldable flex HDI for a high-end sensor application incorporating various plasma-processed microfeatures.
Figure 6.10
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
Microvias by Etching
203
Traditional ceramic-based manufacturing approach for pacemaker circuits.
Figure 6.11
mostly in HTCC or LTCC technology with six to eight conductor layers. After the sintering process is finished, the substrates are cut out by laser and assembled on the first side, including wire bonding or flip chip soldering. Afterward, the substrate is assembled on the backside and additional flexis or cables are connected to the ceramic by soldering or laser welding. Finally, the circuit is functionally tested by in-circuit testing and assembled into the system. This process is very costly and a lot of human interference causes handling defects and low yield. In order to address performance issues as well as cost issues, a new concept for the manufacturing of this kind of circuit has been recommended and implemented. In a flexible approach, the process uses a single-sided assembly where the flexible board is folded up like a butterfly and all the flexible interconnects to the battery and the sensor are integrated directly into the circuit. The substrate is locally rigidized by a suitable carrier material and kept within the large manufacturing panel (12 × 18 in2) by some tabs (Fig. 6.12). Before assembly, the large panel is separated into smaller assembly panels. The attachment of flexible cables is eliminated and the functional test is done using fanned-out test pads arranged in a large pitch pad array, eliminating costly test fixtures and also saving real estate area. After functional test, the circuit is depanelized using a simple cutting tool or by laser cutting and subsequently folded together. When one single joining technique, such as soldering, is used, the assembly can be done directly on the large manufacturing panel using conventional pick-and-place equipment. It is obvious that this approach not only reduces the production cost, but also improves the technical performance of the entire system by minimizing the overall size and weight of the implantable device, resulting in higher acceptance and growing market shares.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
204
Chapter Six
New manufacturing concept based on plasmaprocessed flexible organic substrates.
Figure 6.12
6.4.2.2 High-end mobile communications. The rigid-flexible MCM substrate shown in Fig. 6.13 is used in a high-end military mobile communication system. It consists of four assembly areas connected by integrated flex circuits. The assembly areas are supported by a copper heat sink. The assembly is both C&W and SMT. The large pads around the wire-bonded ICs serve as in-circuit test pads only and do not contain any via holes. The build-up is a 4DC construction, with few signal lines embedded into the GND plane. 6.4.2.3 Missile DSPs. The example in Fig. 6.14 relates to a missile application, where a fast DSP has to be packed into an almost hermetically sealed package. The MCM substrate is a 4D build-up bonded to a CMC carrier. The CMC is a low-CTE material and constrains the substrates very effectively. In addition, it is a good heat conductor and allows high heat dissipation.
Figure 6.13 Rigid-flexible MCM for a high-end mobile communication device.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
Microvias by Etching
205
Fast DSP MCM for a missile application.
Figure 6.14
The build-up is a standard 4D construction with two signal layers on layers 2 and 3. The backside (layer 4) is a full GND layer without signals. The front side contains all pads and VCC. The substrate has almost 2000 internal I/Os, most of which are for wire-bond assembly. In order to seal the circuit quasi-hermetically, a metal lid is soldered onto the surface after assembly and testing. The CMC carrier and the metal lid provide for a very effective diffusion barrier, but humidity may still creep into the cavity from the periphery. Therefore, special diffusion barriers are designed into the inner layers and the almost full copper coverage on the top layers also helps to minimize gas diffusion. Hermeticity tests have shown a very good performance. This type of low-cost package eliminates the need for high-priced Kovar metal can packages with glass feed-through contacts, and also allows a simple connection of the external I/Os to a flexible bus substrate, connecting all the various modules within the electronic system. 6.4.3 Rigid-flexible HDI
The HDI board shown in Fig. 6.15 is the central sensor board for the XMM satellite, the new generation of the x-ray telescope which was launched in 2000. The rigid-flexible HDI is 640 mm long and has a very complex build-up. On both sides of a molybdenum core, which simultaneously provides for rigidity, heat conduction, and CTE matching, two 8D packages are bonded. The actual sensor chip has a dimension of 4 × 4 in2 and is die- and wire-bonded to the central area of the HDI. Since the signals generated by the sensor—which operates at −150°C—are very sensitive, most of the signal lines on the inner layers are designed in the form of real twisted pairs. In order to prevent heat
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Microvias by Etching
206
Chapter Six
Figure 6.15 Complex rigid-flexible HDI substrate for the XMM satellite.
from flowing from the flex tails toward the central sensor area, the copper thickness in the flexibles must be less than 6 µm. The HDI board has been fully approved for the ABRIXAS and XMM mission and is considered one of the most complex HDIs ever produced. 6.5 References 1. Schmidt, W., “Plasma Processed Rigid-Flexible MCMs,” Board Authority, 2(1): 70–74, April 2000. 2. Lau, J. H., and C. Chang, “An Overview of Microvia Technology,” Circuit World, 26(2): 22–32, January 2000. 3. Schmidt, W., “DYCOstrate Technology,” Circuitress, June 1996. 4. Schmidt, W., “A Revolutionary Answer to Today’s and Future Interconnect Challenges,” Proceedings of the Third European Joint Conference (EIPC), Brussels, Belgium, June 17–19, 1992. 5. Schmidt, W., “DYCOstrate Technology: From PCBs to MCMs,” Proceedings of the German EIPC Seminar, Freiburg, Germany, September 23, 1994. 6. Reboredo, L., “Microvias: A Challenge for Wet Processes,” Proceedings of the IPC Expo, S12–1, Long Beach, CA, March 1999. 7. Schmidt, W., “High Performance Microvia PWB and MCM Applications,” Proceedings of the IPC Expo, S17–5, Long Beach, CA, March 1999.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Source: Microvias
Chapter
7 Conductive Paste/Ink-Filled Microvias
7.1 Introduction Due to the fast growth in demands for mobile computing and telecommunication, the technologies of microelectronics packaging require high density, fine pitch, high performance, high reliability, and low cost. In particular, it is becoming more and more difficult for the conventional PCBs with mechanically drilled vias and PTHs to meet the packaging density requirements and to justify their manufacturing cost. To overcome these challenges, new PCB manufacturing schemes for high-density and high-performance multilayer PCBs have been developed recently. These new HDI technologies are categorized as SBU or build-up multilayer (BUM) processes for making laminatebased substrates or PCBs containing microvias formed by laser drilling, photoimaging, or plasma etching. Conductive paste or ink materials may be used to fill the microvias and through-holes to make reliable vertical or z-interconnects.1 The surface metallization may be accomplished either by chemical deposition or by laminating copper foil onto the dielectric surface. A few examples of this category of high-density PCBs include Matsushita’s any-layer inner via hole (ALIVH),2 DuPont’s CB100,1 and Ormet’s OrmeLink.3 The SBU technology with conductive paste/ink-filled microvias can achieve a connection pad density of up to 100 pads/cm2, while the conventional PTHs can reach only 20 pads/cm2. The general fabrication processes for conductive paste/ink-filled BUMs consist of: (1) formation of microvias in individual prepreg layers by laser drilling or photo-
207
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
208
Chapter Seven
imaging, (2) filling via holes with conductive paste/ink materials, (3) lamination of copper foil onto the prepreg with filled microvias, (4) circuitization of copper foil by photolithography, (5) testing of individual layers, (6) lamination of tested individual layers, and (7) circuitization of the outer layers by photolithography. The paste/ink materials used for via filling must have corrosion resistance, electrical conductance, easy adaptability to the existing manufacturing process (e.g., screen-printable), low shrinkage after processing, high strength, good adhesion to PCB materials, and yet low cost. Most such materials comprise metallic particles such as copper, an epoxy resin, a hardener, and, if necessary, a dispersant. The paste/ink having low viscosity and low volatility under high shear should be used to fill microvias and through-holes. 7.2 Conductive Paste and Ink 7.2.1 Conductive paste for via filling4
A conductive paste material usually consists of a conducting filler powder coated with a low-melting-point metal or alloy, a mixture of several thermoset resins, and other minor organic additives. By varying the filler content and resin chemistry, several formulations have been produced to fill via holes with a high aspect ratio. As a common practice, via fill experiments should be performed to demonstrate void-free microstructure with good electrical continuity. Also, various bulk properties such as thermal, electrical, and mechanical properties should be characterized in order to understand the material behavior during via filling as well as field service. 7.2.1.1 Conducting adhesive materials. An electrically conducting adhesive material is made of metallic filler particles loaded in the matrix of a polymer material. The polymer matrix can be either thermoplastic, thermoset, or mixtures of these polymers. Silver-particle-filled epoxy is the most common example of the electrically conducting adhesive materials in use. The silver particles, usually in the shape of flakes, provide electrical conduction via percolation, while the epoxy matrix provides an adhesive bond between the components and a substrate. The silver-filled epoxy material has been long used in electronic applications as a diebonding material,5 where its good thermal conduction rather than electrical conduction property is utilized. Recently, this material has been further developed for applications requiring high electroconduction and fine pitch connection.6–13 The silver-filled epoxy material still has several limitations for electronic applications. These are low electrical conductivity, increase in contact resistance during thermal exposure, low joint
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
209
strength, silver migration, difficulty in rework, and others. Since the silver-filled epoxy material is electrically conductive in all directions, it is classified as an isotropic material. In order to overcome the limitations of the silver-filled epoxy materials, several new formulations have been developed recently for various applications. To meet the reworkability requirements of high-performance applications, such as in an MCM, a reworkable thermoplastic resin has been incorporated with the proper solvent and silver particles.10 Solvent removal from the thermoplastic resin has been carefully controlled during the reflow cycle. Another reworkable thermoplastic conductive paste has also been reported for fine-pitch flip chip applications.7 In this case, by loading fine silver particles in excess of 40 percent by volume, high electrical conductivity superior to the Pb-Sn eutectic solder has been achieved. A new class of conductive adhesive materials has been developed by replacing silver particles with other conducting particles, such as solder particles,14 a mixture of solder and copper,8, 15 tin-coated copper,11, 16 silver-coated copper,17 and others. A solder-polymer composite paste material has been developed by mixing solder powder particles, thermoplastic polymer resin in a volatile solvent, and a fluxing agent.14 Upon reflow, an oxidefree, partially coalesced solder connection is obtained, which is polymer strengthened and reworkable at a low reflow temperature or in the presence of an organic solvent. A hybrid of solder and conductive adhesive joining technologies has been developed to exploit the advantages of both.8 This new conductive adhesive is a mixture of a solder powder, a metal powder of high melting point such as copper, a fluxing agent, a polymer resin, and other additives. Here, the electrical connection is established through transient liquid phase sintering (TLPS) among metal and solder powder as well as to the conducting pads. Promising results have been reported with SMT joints made from the TLPS conductive paste in terms of electrical conductivity, impact strength, and reliability, which are substantially better than those of the conventional conductive adhesives.15 Another improvement has been reported with high-conductivity Pb-free conducting materials. Several formulations have been developed of materials made of a conducting filler powder coated with a low-melting-point metal, a thermoplastic polymer, and other minor organic additives.16, 18 Similar to the TLPS conductive paste, these high-conductivity Pb-free conducting materials also provide metallurgical bonding between adjacent filler particles, and between the filler particles and the contact pads to be joined, in addition to the adhesive bonding from the polymer matrix. Their salient properties have been reported for two different applications; one for high-temperature applications with ceramic substrates, and another for low-temperature applications with organic substrates.19
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
210
Chapter Seven
7.2.1.2 Pb-free conductive materials for via fill applications. A new Pb-free conductive adhesive has been developed for via fill applications with the intent of utilizing the enhanced properties discussed previously. The BiSn-coated Cu powder developed previously18 has been chosen as the conducting filler particles. The BiSn-coated Cu conducting particles are fusible during lamination under heat and pressure. This leads to metallurgical bonds among the conducting particles as well as to the conducting pads, which enhance mechanical and electrical properties of the filled via holes. Since the BiSn coating on Cu powder also provides a protective layer against oxidation on the Cu surface, the longterm reliability of the filled via holes is expected to be superior to the via structure filled with the conventional materials, such as silver-filled epoxy or copper-filled adhesives. Another advantage of the BiSn-coated Cu powder comes from the absence of silver particles in the filled via holes. Silver metal is notorious for corrosion under the condition of moisture and a bias voltage, which often leads to a serious reliability issue in high-performance electronic packages. The resin formulation used in the present conductive adhesive material is unique in low shrinkage and controlled viscosity. The resin system is formulated by mixing several thermoset resins, such as cycloaliphatic-type epoxy, phenoxy polymer, monofunctional limonene oxide, and others. Flux resin is also incorporated into the resin mixture. A controlled viscosity of the resin mixture required for screen printing into a high-aspect-ratio PTH is achieved by adjusting the components of the monofunctional limonene oxide. Several formulations are made by varying the resin mixture as well as the conducting filler content, as listed in Table 7.1. The electrical and mechanical properties of these formulations are measured with the model joints as listed in Table 7.1. The geometry of a model joint and testing methods are given in the literature.19 Table 7.1 lists several examples of the new conductive paste formulations designated, such as BiSn48, BiSn49, BiSn53, and BiSn54. For comparison, it also includes one commercial paste formulation, AgCu01, which contains a mixture of silver and copper particles as a conducting filler in the matrix of an epoxy resin.20 As noted in Table 7.1, the electrical and mechanical properties measured with the new conductive paste formulations are superior to those obtained from the commercial substrates having different characteristics, such as thickness, PTH diameter, aspect ratio, and others. For a thick PCB with a high aspect ratio, a formulation having a high-flow resin such as BiSn49 or BiSn54 is required to fill the vias. For a thin PCB with a small aspect ratio, it is appropriate to use the formulation with a medium-flow characteristics, such as BiSn48. To demonstrate the hole-filling behavior of the new conductive paste formulations, via fill experiments have been performed with two differ-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
211
TABLE 7.1
Electrical and Mechanical Properties of Conductive Adhesive Materials for Via Fill Applications Paste ID
Electrical (Ω) (mean/SD)
Mechanical (lb) (mean/SD)
Remarks
Filler(%)
Resin
Reflow
AgCu01
Ag & Cu (>93)
Epoxy
150°C, 25 psi, 30 min
0.00040 (0.00002)
4.3(0.9)
Commercial
BiSn48
BiSn/Cu (68)
Epoxy Phenoxy Flux
188°C, 50 psi, 30 min
0.00041 (0.00006)
6.7(0.5)
Mediumflow resin
BiSn49
BiSn/Cu (76)
Epoxy Lim-oxide Phenoxy Flux
188°C, 25 psi, 30 min
0.00027 (0.00004)
5.4(0.9)
High-flow resin
BiSn53
BiSn/Cu (77)
Epoxy Lim-oxide Phenoxy Flux
188°C, 25 psi, 30 min
0.00023 (0.00003)
5.1(0.3)
High-flow resin
BiSn54
BiSn/Cu (81)
Lim-oxide Epoxy Phenoxy Flux
188°C, 25 psi, 30 min
0.00018 (0.00002)
3.4(0.3)
Very-highflow resin
ent PCBs—one 0.024 in. thick with a PTH diameter of 0.008 in. (aspect ratio = 3), and another 0.105 in. thick with a diameter of 0.010 in. (aspect ratio = 10). For the thin PCB, the new conductive paste is applied directly by blading and the excess paste is wiped off. For the thick PCB, a coating (0.004 in. thick) of the paste is applied to a polyester carrier film by blading. The carrier film is then laminated into the holes of the PCB by applying a pressure of 500 psi and the use of a mask.21, 22 The via-filled PCB is later cured at 150°C for 30 min. To demonstrate the hole-filling characteristics, the cross sections of the via-filled PCB have been prepared metallographically. Figure 7.1 shows a typical cross-sectional view of the thin PCB filled with the use of blading. A void-free via structure is observed. In the enlarged view in Fig. 7.2, a uniform distribution of the conducting filler particles is noted in the filled via structure. Figure 7.3 shows a typical cross-sectional view of the thick PCB with a high aspect ratio, where the via fill was accomplished by a high-pressure lamination of a carrier layer. Again, a void-free via structure is noted. Figure 7.4 shows an enlarged view of Fig. 7.3, in which a uniform and compact distribution of the conducting filler particles is observed. A Pb-free conductive adhesive material has been developed to fill via holes in the new PCB structure manufactured by the build-up multilayer technology. The new conductive paste material consists of a con-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
212
Chapter Seven
Cross-sectional micrograph of a through-hole filled with a conductive adhesive (BiSn49, listed in Table 7.1).
Figure 7.1
ducting filler powder coated with a low-melting-point metal or alloy, a mixture of several thermoset resins, and other minor organic additives. Via fill experiments have been performed to demonstrate void-free microstructures with good electrical continuity. Bulk properties of the new conductive adhesive materials have also been measured to understand the materials’ behavior during via filling as well as reliability testing.
Enlarged view of the cross section shown in Fig. 7.1.
Figure 7.2
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
213
Cross-sectional micrograph of a through-hole filled with a conductive adhesive (BiSn54, listed in Table 7.1).
Figure 7.3
7.2.2 Conductive ink for through-hole plugging23
STH technology describes a method of creating an electrical interconnect between the top and bottom sides of a printed circuit board. STH production has gained and continues to rapidly gain acceptance worldwide due to its low-cost, reliable, and environmentally friendly process. Even though the technology necessary to produce STH boards is mature, the performance of current through-hole ink relies on different PCBs. The stability of electrical conductivity on exposure to solder
Enlarged view of the cross section shown in Fig. 7.3.
Figure 7.4
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
214
Chapter Seven
baths or to thermal cycling is a predominant issue. This problem is associated with different metal fillers, resin systems, and PCB types. For example, the electrical resistance of the ink on FR-2 substrate gradually increases after each solder bath dip. Fundamental studies have been conducted on the root cause of the hole resistance drifts after solder bath. Thermal mechanical analysis (TMA) and dynamic mechanical analysis (DMA) have been used to characterize the CTE and curing performance of the ink and PCB substrates. The failure mechanism has been proposed and confirmed by designed experiments. Experimental results demonstrated that hole resistance drift on FR-2 substrate is caused by several factors. First, the higher thermal expansion of the substrate itself stretches the coating layer. Second, the continued curing makes the resin matrix fixed at a higher temperature. The final factor is the CTE mismatch between the conductive ink and the PCB substrate. STH technology describes a method of creating an electrical interconnect between the top and bottom sides of a printed circuit board. This method involves screen printing a conductive paste into drilled holes and then drying and curing the paste. The paste can be filled with silver, copper, or any combination of conductive metals. STH production continues to rapidly gain acceptance worldwide for several reasons. The selling price of an STH-produced paper phenolic board is 30 percent to 40 percent less than that of an electroless-copper-plated epoxyglass board. The STH process is environmentally more friendly than plated through-hole processes. The technology necessary to produce through-hole boards is mature and not excessively complicated. The cost of the equipment is very low, and equipment is most often already available from a printed circuit board producer. Besides, the reliability of STH boards meets or exceeds the requirements for many applications. Even though the technology necessary to produce STH boards is mature, the STH ink needs to be improved for the final product reliability. The vast majority of the PCB through-hole inks in the marketplace today are based on modified phenolics. The stability of electrical conductivity on exposure to solder bath or thermal cycling is a predominant issue for the current products on FR-2 board. Reduction of the STH ink cost is another major issue for the current products. These problems are associated with different metal fillers, resin systems, and printed circuit boards. Fundamental studies have been conducted on the root cause of the two issues. The understanding of the failure mechanism leads to new product development.24 7.2.2.1 Process for through-hole connection. Through-hole connections can be applied to single- or double-sided PCB materials such as FR-2, FR-4, and CEM-1. The general process for through-hole connections is as
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
215
follows. After etching, the via holes can be drilled. The most frequently used hole dimensions are 0.5 to 1.0 mm in diameter. The PCB substrate is usually 1.0 to 1.6 mm thick, with copper pads that are generally 0.8 to 1.2 mm larger than the hole diameter. The printed silver dots are generally 0.4 to 0.7 mm larger in diameter than the hole. Drilled holes are recommended, since punching does not provide a smooth enough surface to allow consistent deposition of ink. Furthermore, the reliability of punched hole boards is inferior with respect to resistance stability and silver migration. A standard copper cleaning process has to be done before the through-hole print to remove any copper oxidation and contamination. After cleaning, the board must be properly dried or the moisture trapped in the holes will cause voiding. The through-hole conductive ink is screen-printed into the holes. Three generations of printing techniques are now common, and several variations of these have been developed by many companies. The oldest and most traditional is the folded-over squeegee technique, where high squeegee pressures fold the squeegee onto the screen. The second, newer, and increasingly more popular technique is the beveled squeegee technique. The third and newest technique uses a 20-mm-wide squeegee and a very small printing angle. All methods are used with a high degree of success by many companies. Drying and curing refer to different processes. Drying refers to the removal of solvent prior to the actual curing cycle, during which resins cross-link and form the final network. A final coating of solder mask is applied to cover the printed holes in order to provide protection from oxidation and physical and/or chemical damage. 7.2.2.2 Electrical resistance test vehicle. The materials used for the electrical resistance tests are commercially available Electrodag PR408 and PR-011 silver polymer thick film ink for through-hole printing. The conductive paste is homogenized properly and may be diluted to the required process viscosity. Several tests should be conducted to identify the mechanisms responsible for the unstable resistance of the ink after solder bath. Sheet resistance test vehicle preparation (Fig. 7.5) involves printing the material on a glass substrate and then drying and curing it under appropriate conditions. The sheet resistance in Ω/square at 25 µm of a particular conductive track can be calculated from Eq. (7.1) by measuring the actual resistance R of the conductive track, the number of squares N involved, and actual coating thickness t, as follows:
Sheet resistance = (R × t)/(N × 25) (Ω/square/25µm)
(7.1)
Note that the number of squares N equals length divided by width of the coating layer.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
216
Chapter Seven
Figure 7.5
Test vehicle for sheet
resistance.
The hole resistance is measured over a row of several through-hole connections (Fig. 7.6) using a digital multimeter. For measuring the resistance of one hole, four-point measuring equipment is needed to overcome the contact resistance between the leads and copper circuit. All samples should be dried for 30 min and then cured at 175°C for 30 min to mimic the manufacturing cure timing. The initial resistance Ro is measured once the samples equilibrate to room temperature. Then the samples are dipped into a solder bath at 250°C for 10 s. The resistance Rt should be measured after the samples cool down to room temperature. 7.2.2.3 Coefficient of thermal expansion. CTE measurement of a cured formulation and PCB boards is performed on a thermomechanical analyzer. The CTE of PCB substrate should be measured along three different orientations. The x- and y-directions are along the surface of the board, while z is perpendicular to the board surface and along the through-hole direction. In order to achieve the minimum thickness requirement of TMA without voids in the sample, multilayer coatings may be applied for through-hole ink. Each individual drying is conducted at 70°C after a new coating layer is applied, and final curing at 150°C is performed after the total coating layers reach 2 mm thick. The CTE should be measured from −50 to 200°C at a heating rate of 5°C/min. 7.2.2.4 Dynamic moduli and curing characterization. Curing is studied by monitoring changes in dynamic moduli as a function of temperature
Figure 7.6
Test vehicle for hole resistance.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
217
and time using a dynamic mechanical analyzer. The preparation of a specimen used for the DMA test should be the same as that for the TMA test except for the size. The measurement is performed in a singlecantilever mode under 10-Hz sinusoidal strain loading. Heat should be applied from room temperature to 200°C at a heating rate of 5°C/min. 7.2.2.5 Reliability testing. Figure 7.7 shows the results of electrical resistance change after solder bath at 250°C for PR408 on FR-2 and FR-4 boards. The reliability performance is quite different for FR-4 boards compared with FR-2 boards when the samples are cured at 150°C for 30 min. On FR-4 boards, the hole resistance drops a little after the first solder dip, then remains stable when the specimen experiences further solder dips. On FR-2 boards, instead of maintaining stable resistance after the first solder dip, the hole resistance gradually increases. This unstable resistance makes the through-hole conductive ink finally fail the solder bath reliability test after several dips. In order to understand the failure mechanism of current formulations of FR-2 boards, the physical properties of the through-hole ink and PCB substrates are characterized. CTE values as well as softpoints of through-hole ink and PCB substrates are listed in Table 7.2. It has been observed that CTE is similar for FR-2 and FR-4 along the x- and y-directions. However, the CTE value is significantly larger for FR-2 than for FR-4 along the through-hole z-direction. Comparing the CTE value in the z-direction between the through-hole ink and substrates, it was found that the CTE of through-hole ink is very close to that of FR-4, but much smaller than that of FR-2. The softpoint of FR2 is lower than that of FR-4, but both are much higher than the softpoint of conductive ink when the samples are cured at 150°C for 30 min. However, the softpoint of the conductive ink increases after it experiences heating up to 200°C. This increase in the softpoint of con-
Figure 7.7
The effect of solder bath on hole resistance.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
218
Chapter Seven
ductive ink indicates that further curing occurs at elevated temperatures. The curing at elevated temperatures should be further investigated by DMA to characterize the dynamic storage modulus changes with temperature for PR-408 and PR-011. The initial run indicates that the glass transition temperature of PR-408 is about 50°C after the sample is dried at 70°C for 30 min followed by curing at 150°C for 30 min. Notably, the storage modulus increases when the sample is held at 200°C for 10 min. Then the same specimen is tested for the second time. At this time, both storage modulus and glass transition temperature have increased. The same phenomenon is observed on PR-011 formulations based on the same resin system. The DMA results confirm that further curing occurs at elevated temperatures. Based on the observed failure phenomenon and characterized physical properties, a failure mechanism has been proposed. Figure 7.8 schematically illustrates the failure mechanism due to the CTE mismatch and continued curing. Corresponding dimension changes of conductive ink and PCB substrates at different stages are shown in Fig. 7.9. When PCB substrate coated with through-hole ink is dipped into solder bath, the PCB substrate stretches due to thermal expansion. Since the glass transition temperature of the ink is below that of the PCB substrate, the coating layer will expand at the same level. The conductive ink on FR-4 is stretched much more than that on FR-2 substrate since the CTE of FR-2 is much higher than that of FR-4. Assuming that the relative dimension change at 0°C is zero, then the thermal expansion of the FR-2 board is about 60,000 ppm while that of FR-4 is about 16,000 ppm based on CTE measured by TMA. When the temperature cools down to the glass transition temperature of the ink, the resin matrix is fixed. If no further curing occurs, the through-hole conductive ink coated on the hole should shrink back to its original state with the PCB substrate when it reaches room temperature. Therefore, TABLE 7.2
CTE (ppm/°C)
CTE of Through-Hole Inks and PCB Substrates PR408
PR011
FR-2
FR-4
1st run −50 to 200°C x-
48
58
19
19
y-
48
58
20
17
z-
48
58
115/279
44/78
0°C
64°C
100°C
Softpoint
10°C
2nd run −50 to 200°C x-, y-, zSoftpoint
50
54
No change
No change
175°C
175°C
No change
No change
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
219
the hole resistance, determined by the volume fraction of the conductive fillers, should keep the same value before and after solder bath. However, due to the further curing of the resin system, the glass transition temperature of the ink increases; thus, the resin matrix is fixed at a higher temperature as shown in Fig. 7.9. When the temperature further cools down to room temperature, the ink will shrink based on its own CTE below Tg instead of shrinking along with the board. The resin matrix fixed at higher Tg causes the final resin matrix after the solder bath to be larger than that before the solder bath. In other words, the volume fraction of the conductive ink becomes smaller. As a consequence, resistance increases. Since the CTE of FR-4 is much smaller than that of FR-2 and the CTE mismatch between the ink and FR-4 is also less than that for FR-2, the relative dimension change before and after solder bath dip on FR-4 substrate is much smaller than on FR-2 substrate. For example, the relative dimension change on FR-2 is about 30,000 ppm, while that on FR-4 is about 1,600 ppm assuming Tg is about 50°C and 175°C before and after the solder bath, respectively. In order to confirm the proposed failure mechanism, the sample is cured at 250°C for 30 min to guarantee that no further curing occurs during solder bath at 250°C. Then the solder bath reliability test is conducted. Since there is no further curing happening during solder dip, the resistance should stay stable before and after solder bath based on the assumption. The experimental results in Fig. 7.10 show that resistivity stays stable after several solder dips for both FR-4 board and FR2 board. This result supports the proposed failure mechanism. The electrical resistance of the through-hole conductive ink on FR-2 substrate gradually increases after each solder bath dip. But the hole resistance is stable on the FR-4 substrate. Experimental results demonstrate that a hole resistance drift on FR-2 substrate is caused by several factors. First, the higher thermal expansion of the substrate itself stretches the coating layer. Second, the continued curing of the ink during the solder bath test causes the resin matrix to become fixed at higher temperatures. The final factor is the CTE mismatch between the conductive ink and PCB substrate. FR-2 substrate has a much larger CTE than FR-4. The CTE mismatch between conductive ink and FR-2
Figure 7.8 Schematic diagram of dimension change under solder bath dip.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
220
Chapter Seven
Relative dimension change of conductive inks and PCB substrates.
Figure 7.9
is much bigger than that between ink and FR-4. Current PR-408 and PR-011 formulations will continue to cure at elevated temperatures. As a consequence, the volume fraction of conductive filler becomes smaller after solder dip, which causes the resistance increase. 7.2.3 Example of application1
CB100 is a screen-printable paste made of silver, copper, and epoxy. Figure 7.11a shows a stacked via over filled PTH, and Fig. 7.11b shows an integrated IC-PCB assembly with the CB100 conductive via plug. CB100 is usually stencil-printed in the plated or unplated throughholes. After drying and curing, the plugged through-holes are planarized and plated to make them solderable. The design rules for CB100 are: aspect ratio = 1:1 to 6:1 with vacuum assist; via size = 6 to 25 mil (152 to 635 µm); and core thickness = 6 to 85 mil (152 to 2159 µm). The CTE is less than 35 ppm/°C. The CB100 assembly process is as follows:
Hole resistance change after solder bath with sample cured at 250°C for 30 min.
Figure 7.10
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
221
(a)
(b)
(a) Stacked via over filled PTH with DuPont’s CB100. (b) Fully integrated IC-PCB with redistribution layer, controlled impedance, thermal dissipater, buried capacitor/resistor, and EMI shielding.
Figure 7.11
■
Drill through-holes on the double-sided copper clad substrate.
■
Screen/stencil-print CB100 into the through-holes.
■
Dry and cure the via-plugged CB100.
■
Scrub and planarize the surfaces.
■
Plate the filled board with about 0.3 to 0.5 mil to enhance electrical conductivity and solderability. (With a multilayer core, the throughhole is first flash-copper-plated with a minimum of 0.1 mil copper to ensure interplane connection.)
■
External flash-electroplate copper.
■
Form wiring patterns on both sides of laminate by printing and etching.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
222
Chapter Seven
There are some qualification data for the CB100 ViaPlug.20 It can be seen that the material can pass 1000 temperature cycles (−65 to 125°C) and pass 5 solder dips at 286°C.
7.3 Any-Layer Inner Via Hole (ALIVH)2 Matsushita has developed a unique stacked-type substrate technology called ALIVH. Laser ablation (currently CO2 laser) and conductive paste (with Cu particles/epoxy carrier) are used for the formation of interconnects. It is reported that Matsushita’s share in the Japanese cellular phone market has risen to 60 percent with the introduction of ALIVH substrates (Fig. 7.12). The ALIVH process is very popular in Japan. However, in order to gain market share, ALIVH must migrate to other fabrication facilities outside Japan. The ALIVH technology has the capability to carry HDI processes well into the next several generations of build-up multilayer requirements. As with all HDI processes, the cost of additional processes and special materials must be traded off against the benefit of greater circuit density and other metrics such as time to market and reliability. There could also be a “pull” effect from OEMs whose future designs require the capabilities of a process not constrained by conventional plating processes, where aspect ratio and plating distribution do not impede circuit density. In the future, it may also be possible to eliminate the intermediate pads and create structures that have even greater routing density.
7.3.1 Classification of ALIVH
The three versions of the ALIVH process, currently available in Japan, are designated ALIVH, ALIVH-B, and ALIVH-FB. Each has the capability of providing high-density interconnect capability for different packaging complexities and market segments required by
(a)
(b)
(a) ALIVH substrate for mobile phones. (b) Cross-sectional view of a typical ALIVH substrate.
Figure 7.12
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
223
OEMs.25 All three ALIVH processes use laser drilling to create microvias in individual sheets of prepreg. The holes are subsequently screen-filled with a conductive paste, which creates a conductive path from one side of the prepreg to the other. Internal layers that are equivalent to conventional inner-layer cores are created in an extra lamination step by laminating foil to the prepreg and then completing a standard print-and-etch process sequence to create the circuit features of each layer pair. The fabrication process concludes by adding additional layers of dielectric material (also with conductive paste in the holes) and the outer-layer foil before laminating the package together and completing a print-and-etch process that creates the outer-layer circuit features and a thick multilayer structure. The standard ALIVH structure is best suited for the smaller/lighter product segments in consumer electronics (over 18 million cell phones have been manufactured with this process). The ALIVH-B and -FB processes are focused on the motherboard, chip-scale packaging, and direct chip attach segments of the industry. The -B and -FB processes are competing for market share where more complex HDI board designs are required and where product reliability is a key metric. ALIVH structures do not use conventional PCB substrates for rigidity like some of the high-volume build-up multilayer structures using photoimageable dielectrics or resin-coated copper. The common thread in the ALIVH processes is the use of an Aramid/epoxy prepreg and a conductive paste to provide electrical connection. Blind and buried vias are standard ALIVH features, but the competitive advantage is that these vias can be connected to any other layer in the stack-up. A stacked, solid via-on-via or via-on-pad replaces conventional drilled, lasered, or imaged microvias and electroplating. There are no aspect ratio constraints. There is also no hole plugging required after solder mask in the ALIVH processes. 7.3.2 Characteristics and advantages
The premier benefit of ALIVH is described in its name. Designers can connect from any layer to any other layer (Fig. 7.13)—a capability that is not available in other build-up structures. Take a six-layer design, for example. Connections can be made from one layer to any other layer (say, from layer 2 to layer 5) with no aspect ratio constraints (as for electroplating). This capability will change the way designers create a structure. Design flexibility is increased and overall layer count is reduced because of the routing opportunities created when individual layers are manufactured one at a time. In addition, by laser drilling the holes and screening the conductive paste into each layer of prepreg
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
224
Chapter Seven
Figure 7.13
ALIVH—any layer to any other layer.
prior to the final lamination step, each layer can be electrically tested and repaired or replaced, if necessary. The ALIVH inner layers are “known-good” before the outer layer is created. This is a distinct advantage in yield compared to typical build-up processes where the substrate is at risk each time it makes one of the required multiple passes through the processes required to create the build-up structure. ALIVH also has a unique attribute from an environmental standpoint; since it is essentially a “dry/mechanical” process requiring only inner-layer FAB to print and etch the circuitry (no electroless copper, electroplating, or final strip and etch), much of the wastewater treatment and support cost associated with the high-maintenance outerlayer processes is eliminated. Because ALIVH is less complex compared to some other alternatives, it should also be less expensive. 7.3.3 Design and tooling26
In the ALIVH processes, the ability of the design systems to capture the unique hole formation pattern on each prepreg layer and match it to the corresponding foil layer could be a challenge. There are at least two systems currently available that can support ALIVH designs. In addition, fully utilizing the via-on-via and via-on-pad capabilities will require extra effort on the part of the designers to learn how to create new products with another degree of freedom. Greater design flexibility is obtained because blind and buried via connections are not constrained by the mechanical operations or electroplating aspect ratios, and outer-layer traces are created by a print-and-etch process, eliminating the effects of plating distribution.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
225
Table 7.3 shows some of the minimum design features available with ALIVH. It should be noted that circuit density is not a significant advantage in the ALIVH process because these feature sizes can be obtained by other HDI processes. The tooling processes prior to manufacturing will need modification and additional documentation to address the multiple passes through inner-layer FAB and lamination. 7.3.4 Features of materials
The ALIVH prepreg uses a nonwoven Aramid-reinforced cloth impregnated with a high-Tg (168 to 180°C) epoxy resin. The resin content can be varied somewhat to meet other design trade-offs. This family of prepregs has a lower in-plane CTE, ranging from 6 to 10 ppm/°C versus ∼15 ppm/°C for standard FR-4. Also, when compared to a conventional FR-4 multilayer with woven glass, a similar structure using ALIVH can be 30 percent to 50 percent lighter. In ALIVH processes conventional copper electroplating of the hole walls is replaced with uniform via plugging using a conductive paste that has copper particles embedded in an epoxy carrier. Copper particles vary in size and are as small as 4.45 µm in the high-end ALIVHFB process. The conductivity variation using the conductive paste is ⫾20 percent, including the microvias, and dielectric resistance variation is greater than 1 × 107 Ω after testing. The dielectric constant Dk ranges from 4.1 at 1 MHz to 3.5 at 1 GHz. TABLE 7.3
Design Minimums of Standard ALIVH, ALIVH-B, ALIVH-FB Features
Lines
Spaces
Pads
100 µm (4 mil) 100 µm (4 mil)
400 µm (16 mil) 400 µm (16 mil)
50 µm (2 mil) 50 µm (2 mil)
250 µm (10 mil) 250 µm (10 mil)
25 µm (1 mil) 25 µm (1 mil)
150 µm (6 mil) 150 µm (6 mil)
Standard ALIVH Outer layer Inner layer Via diameter = 200 µm (8 mil) Dielectric thickness: 50–125 µm (2–5 mil)
100 µm (4 mil) 100 µm (4 mil)
Outer layer Inner layer Via diameter = 125 µm (5 mil) Dielectric thickness: 50–125 µm (2–5 mil)
50 µm (2 mil) 50 µm (2 mil)
ALIVH-B
ALIVH-FB Outer layer Inner layer Via diameter = 50 µm (2 mil) Dielectric thickness: 12.5 µm (0.5 mil)
25 µm (1 mil) 25 µm (1 mil)
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
226
Chapter Seven
Since ALIVH processes are different from conventional processes, extra development time has been spent to ensure that critical risk factors for OEMs have been addressed. In these ALIVH processes to enhance the bond strength between the conductive paste and the copper foil, a new surface treatment process for the foil was developed. In addition, modifications to the copper particle geometry, paste viscosity, and epoxy binder system were also made to ensure reliability and assembly survivability. One of the known disadvantages of Aramid-epoxy resin systems is moisture absorption. A special formulation of prepreg to reduce the effects of moisture has been developed in Japan. North American suppliers may also offer similar low-moisture-absorption materials. Also, most of the applications for ALIVH will be thin, low-layer-count, highdensity structures because the z-axis expansion of Aramid-epoxy is worse than that of FR-4. 7.3.5 Manufacturing processes 7.3.5.1 Basic procedures. The fabrication process flowcharts for ALIVH substrates are shown in Fig. 7.14. The basic procedures are illustrated as follows. ■
The nonwoven Aramid-epoxy prepreg is used as a substrate material. The B-staged Aramid-epoxy sheets are drilled out to form via holes using a CO2 laser for the electrical connection between conductive layers.
■
The via holes are filled with the via conductor paste. The via conductor paste consists of copper particles and a thermosetting resin. Two copper foils and the via-filled Aramid-epoxy prepreg are stacked to be laminated, sandwiching the aramid-epoxy prepreg between two copper foils with no gap. The lamination and curing of the aramidepoxy prepreg are performed under a pressure and a temperature. Wiring patterns are formed by etching the copper foil layers.
■
The other via-filled Aramid-epoxy prepregs are stacked on both sides of the wiring-patterned Aramid-epoxy sheet. Furthermore, two copper foils are stacked on both sides of the stacking laminates. Lamination is performed under a pressure and a temperature. Finally, the wiring patterns of both sides of laminate are formed by etching
7.3.5.2 Fabrication of ALIVH. The manufacturing process is different from conventional circuit board fabrication in a number of ways, but, aside from requiring the use of unique materials (conductive paste and nonconventional prepreg) and multiple passes through core processes and typical HDI equipment (laser drill), the ALIVH process can be
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
(a) Figure 7.14
227
(b)
Process flow chart for (a) ALIVH and ALIVH-B, and (b) ALIVH-FB.
integrated into a conventional process flow. An assumption is made that there is adequate excess capacity in the inner-layer FAB and lamination processes or sufficient space to expand capacity to support these and other special process steps. At the tooling process, each layer must now be analyzed as having both a copper component and a prepreg component. Depending on the stack-up, one or more lamination steps may be required to create the finished product. A decision is then required as to which layers have copper patterns (signal or power/ground), and these layers are routed through lamination and back to inner-layer print and etch. A drilling machine using a CO2 laser—which has been modified to use a mask or aperture system as part of the optical path to control the characteristics of the beam—is directed by galvanic mirrors to cover an area of approximately 400 mm2 in each step. Inner-layer fabrication begins with CO2 laser drilling of the Aramidepoxy prepreg in the pattern of the conductive pathways for each layer. All of the prepreg pieces for the complete stack-up are processed through a screen-printing operation to push the conductive paste inside the laser-drilled holes. If the prepreg is between the component layer and layer 2, or the circuit layer and layer n−1, these prepreg pieces (uncured) are set aside until the package is laminated later in the process. Those
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
228
Chapter Seven
inner-layer prepreg pieces that are the equivalent of inner-layer cores are sent to lamination to have copper foil attached to both sides. These “cores,” which now have conductive pathways from side to side, are then processed through conventional inner-layer print-and-etch processes (clean, laminate resist, expose, DES, and AOI) to create the circuit/plane and pad patterns required by the design. Once this step is completed, the finished core(s) and the prepreg pieces for the outer layers—with conductive paste applied—are sent back into lamination to complete a conventional layup with a second application of foil and a second lamination cycle. The outer-layer image is created using an inner-layer print and etch process. Any remaining process steps (solder mask, etc.) are completed using standard processes. 7.3.5.3 Fabrication of ALIVH-B. The basic manufacturing process for ALIVH-B is the same as that for ALIVH, and the CO2 laser system with a mask in the optional path is the same. However, to achieve the lines and spaces and hold registration, additional modifications may be required in the image transfer and tooling processes. Image transfer may require a collimated light source, a thinner dry-film resist, film alignment capability at exposure, and/or a ferric chloride etchant with spray pattern enhancements. Registration from layer to layer may need to be improved with process control and designed experiments or a more robust tooling system. 7.3.5.4 Fabrication of ALIVH-FB. The manufacturing process for ALIVH-FB begins with the creation of the necessary support structure (the “substrate”) using the processes and design rules of ALIVH-B (see the preceding text). The ALIVH-FB build-up process begins with the creation of the outermost copper layers on a carrier material, such as aluminum. This can be accomplished either additively or using a subtractive process. In the additive process, for lines/spaces at 25 µm (1 mil) or less, photoresist is applied to the carrier, and the image is transferred using a projection mask, then developed and electroplated and the resist stripped. The dielectric for the build-up layers is a double adhesive polyimide film that is 12.5 µm (0.5 mil) thick. All of the polyimide layers are drilled using a YAG laser with an optical mask set for 50 µm (2 mil), and these vias are filled with conductive paste using the screen-printing technique common to all ALIVH processes. Next, the imaged carrier is aligned with one side of the polyimide film and copper foil is matched with the other side. This structure is laminated together. During lamination, the polyimide fills in around the patterned copper on the carrier side, using the carrier as a continuous, flat barrier. The copper foil bonds to the polyimide on the opposite side. After pressing, the copper foil side is patterned using standard inner-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
229
layer print-and-etch techniques. If more than one layer of FB build-up is required, the carrier is etched away and the first-pass lamination steps are repeated before the copper foil is patterned. FB layers are aligned with the Aramid-epoxy substrate layers created previously and the package is laminated a final time to create the competed FB structure. The carrier layers are etched away in the final processing step before finishing. 7.3.6 Electrical performance27
In order to design packages in the gigahertz frequency range, accurate equivalent circuits such as an interstitial via hole in an ALIVH substrate and a through-hole in an FR-4 substrate were extracted using a resonant method from 1 to 10 GHz. The ALIVH substrate is a highwiring-density multilayered organic substrate with inner via hole structure. The resonant method uses the principle that the resonant frequency of a resonator is perturbed by the connection of a lumped element. The via hole was described as a single π-type network model: a series inductance and two parallel capacitances. Consequently, it was confirmed that signal reflections at the via hole were perfectly suppressed by an optimization of geometric dimensions of the via hole, such as the size of a ground plane cutout. Based on these results, the ALIVH substrate was found to be good enough to apply to high-speed systems up to 10 GHz. The via holes in the ALIVH substrate and the FR-4 substrate were characterized by actual measurement using the resonant method in the high frequency range. The influence of the radius of the ground plane cutout and the height of the via hole was also evaluated. Consequently, it was confirmed that the signal reflections at the interstitial via hole were perfectly suppressed by an optimization of geometric dimensions of the interstitial via hole such as size of the inner ground plane cutout. Based on these results, the ALIVH substrate was found to be good enough to apply to high-speed systems up 10 GHz. 7.3.6.1
Geometric influence
A reference resonator and target resonator with different radius r of the inner ground plane cutout in the ALIVH substrate were fabricated, as shown in Fig. 7.15. This is a cross-sectional view of the target resonator with r = 0.45 nm and h = 448 nm. The radius of the via hole and the via land were 0.1 mm and 0.2 mm, respectively. The thickness of the inner ground plane was 18 µm. The resonant characteristics were measured using an HP8719D network analyzer from 1 to 10 GHz frequency. Measure values Xseries and Xshunt were inductive and capacitive, respectively. In Figs. 7.16 and 7.17, the equivalent series inducCutout size.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
230
Chapter Seven
Cross-sectional view at the center region of the target resonator with four stacked vias in the ALIVH substrate.
Figure 7.15
Figure 7.16 Equivalent series inductance of the via hole as a function of the resonant frequency for different radii of the inner ground plane cutout (ALIVH).
tance and shunt capacitance of the via hole are shown as a function of resonant frequency from 1 to 10 GHz for the radius r = 0.3 mm, r = 0.45 mm, r = 0.7 mm, and r = 1.2 mm of the inner ground plane cutout. The influence of the radius r of the inner ground plane cutout is shown in Figs. 7.18 and 7.19. The equivalent series inductance and the equivalent shunt capacitance were L = 0.167 nH and C = 0.084 pF, respectively, for radius r = 0.45 mm of the inner ground plane cutout. The equivalent series inductance increases gradually with the radius r. On
Figure 7.17 Equivalent shunt capacitance of the via hole as a function of the resonant frequency for different radii of the inner ground plane cutout (ALIVH).
Equivalent series inductance of the via hole as a function of the radius of the inner ground plane cutout at 1 GHz (ALIVH).
Figure 7.18
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
Figure 7.19 Equivalent shunt capacitance of the via hole as a function of the radius of the inner ground plane cutout at 2 GHz (ALIVH).
231
Equivalent series inductance of the via hole as a function of the height of the via hole for different radii of the inner ground plane cutout (ALIVH).
Figure 7.20
the other hand, die equivalent shunt capacitance decreases gradually with the radius r. Via hole height. In order to evaluate the influence of the height of the via hole, a reference resonator and target resonators with height h = 224 µm of the via hole in the ALIVH substrate were fabricated. In Figs. 7.20 and 7.21, the equivalent series inductance and shunt capacitance of the via hole are shown as a function of resonant frequency from 1 to 6 GHz for the radius r = 0.3 mm, 0.45 mm, and 0.7 mm of the inner ground plane cutout. The comparison for the equivalent series inductance and shunt capacitance with different height h of the via hole is shown in Table 7.4. The equivalent series inductance increases with
Equivalent shunt capacitance of the via hole as a function of the height of the via hole for different radii of the inner ground plane cutout (ALIVH).
Figure 7.21
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
232
Chapter Seven
TABLE 7.4 Comparison of the Equivalent Series Inductance and Shunt Capacitance with Different Heights of the Via Hole
h (µm)
r (mm)
L (nH)
C(pF)
224
0.45
0.070
0.093
448
0.45
0.167
0.084
the height h. On the other hand, the equivalent shunt capacitance decreases slightly with the height h. Through-hole in an FR-4 substrate. The high-frequency properties of the through-hole in PR-4 substrate with a conventional four-layered structure were evaluated as shown in Fig. 7.22. The figure is a cross-sectional view of a center region of the target resonator in die FR-4 substrate. A reference resonator and target resonators with different radius r of the inner ground plane cutout were fabricated. The radii of the throughhole and the through-hole land were 0.15 and 0.3 mm, respectively. The total thickness of the substrate was 1.6 mm. The thickness of the inner ground plane was 35 µm. In Figs. 7.23 and 7.24, the equivalent series inductance and shunt capacitance of the via hole are shown as a function of resonant frequency from 1 to 6 GHz for the radius r = 0.45 mm, 0.55 mm, 0.8 mm, and 1.3 mm of the inner ground plane cutout. The equivalent series inductance and shunt capacitance were L = 0.685 nH at 1 GHz and C = 0.248 pF, respectively, at 2 GHz for radius r = 0.45 mm.
7.3.6.2 Simulation analysis. In order to validate the signal response at the die via hole, the calculation of die reflected step waveforms was carried out using an HP85150 microwave design system (MDS). The simulated circuit model shown in Fig. 7.25 represents the π-type network model of the via hole connected to ideal transmission lines with a series resistor in order to match the characteristic impedance of the die transmission line. Figure 7.26 shows the time domain pulse response for the reflected waves for the radius r = 0.3 mm, 0.45 mm, and 1.2 mm of the inner ground plane cutout. Rise time of the input step waveform with 1-V swing was 45 ps. Propagation delay time in the ideal trans-
Figure 7.22 Cross-sectional view at the center region of the target resonator with conventional PTH in the FR-4 substrate.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
Equivalent series inductance of the through-hole as a function of the resonant frequency for different radii of the inner ground plane cutout (PTH in FR-4).
Figure 7.23
233
Figure 7.24 Equivalent shunt capacitance of the through-hole as a function of the resonant frequency for different radii of the inner ground plane cutout (PTH in FR-4).
mission lines was 50 ps. The element values to perform this calculation are shown in Table 7.5. The waveforms varied significantly according to the radius of the ground plane cutout. Figure 7.27 shows the magnitude of |S11| for the radius r = 0.3 mm, 0.45 mm, and 1.2 mm of the inner ground plane cutout. The reflections were 3.3 percent for radius r = 0.45 mm and 14 percent for radius r = 0.3 mm and 1.2 mm at 10 GHz. 7.3.6.3 Comparison and discussion. Comparison of the design specification of the ALIVH and build-up substrate is shown in Table 7.6. Though there are many differences in the geometry and dimensions between the ALIVH and build-up substrates, they perform the same functions. The via hole that connected each surface of the substrate was noted. Since the geometry of the ALIVH substrate is very similar to the geometry in the previous section, the inductance of the four stacked via holes is about 0.2 nH. Build-up substrate includes the FR-4 substrate as a core layer. Since the thickness of the core layer in the build-up substrate is half of that in the previous section, the inductance of the through-hole is about 0.4 nH. Therefore, it is concluded that the inductance of the via hole in the ALIVH substrate is half of that in the build-up substrate.
Figure 7.25
Circuit model for simulation.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
234
Chapter Seven
Figure 7.26 Reflected pulse waveform for different radii of the ground plane cutout.
7.3.7 Reliability testing2
In the literature, it has been reported that the ALIVH substrate can pass 1000 thermal cycles for the temperature range from −55 to 125°C. The reliability test data of ALIVH and ALIVH-B are presented in Tables 7.7 and 7.8, respectively. The reliability testing for the FB structures is still ongoing. The available data show that the pressure cooker test has been completed at 121°C, 2 atm for 480 h. An atmospheric thermal shock test from −40 to 80°C, with a 30-min cycle time, has run for 1500 cycles. In all cases, the resistance of the 50-µm (2-mil) holes remains stable. 7.3.8 Applications
The basic ALIVH process should be considered for products requiring lightweight, small, low-layer-count, thin profiles and high reliability. Many cell phones currently being manufactured in Japan use this technology. The ALIVH-B process capability was developed for the motherboard, chip-scale package, and multichip module market segments of the computer products sector. As you can see from the design rules, the ALIVH-B process is very competitive with the most advanced HDI processes. The ALIVH-FB process is designed for direct chip attach applications. It is designed to address the issues of coplanarity in assembly for this TABLE 7.5
Electrical Parameters Used for Simulation r (mm)
L (nH)
C (pF)
0.3
0.108
0.134
0.45
0.147
0.081
1.2
0.269
0.019
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
235
Magnitude of |S11| for the radii of r = 0.3 mm, 0.45 mm, and 1.2 mm of the inner ground plane cutout.
Figure 7.27
industry segment. The ALIVH-FB process is the equivalent of a build-up multilayer process using a conventional FR-4 substrate and laminating photoimageable dielectric or resin-coated copper layers to the outside. In this case, the ALIVH-FB layer or layers are added to a “substrate” that is one or more layers manufactured using the ALIVH-B process described previously. The FB process requires both CO2 and YAG laser capability, additional image transfer capability, and implementation of an etchable carrier system for the build-up layers. However, the breakthrough in the FB process is the embedding of circuitry into the outermost dielectric layer—which is 12.5-µm (0.5 mil)-thick polyimide film using the carrier sheet as a barrier. The resulting surface coplanarity of the structure (measured at 1 µm over 9 mm in prototype volumes) is capable of meeting the assembly process requirements for direct chip attachment. 7.4 OrmeLink Parallel Build Technology While current leading-edge products have achieved 495 leads/in2 (76.7 leads/cm2), projections for the year 2000 show a need for 17,760 TABLE 7.6
Comparison of Design Specifications Between ALIVH and Another Build-up Substrate ALIVH
Build-up
Layer structure
4
2-2-2
Substrate thickness
0.4 mm
0.8 mm (core layer)
Via diameter
0.2 mm
0.3 mm (core layer)
Land diameter
0.4 mm
0.6 mm (core layer)
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
236
Chapter Seven
TABLE 7.7
Reliability Test Results of Standard ALIVH Results
Conductivity
High-temperature storage
Test description
150°C/1000 h
Test conditions
Pass
N/A
Low-temperature storage
−65°C/1000 h
Pass
N/A
High humidity
60°C/90% RH/1000 h
Pass
Pass
High humidity + load
60°C/90% RH/15VDC/ 1000 h
Pass
Pass
Thermal cycling
−65°C to 125°C/100 cycles
Pass
N/A
Hot oil
260°C (10 s) to 20°C (10 s)/ 10 cycles
Pass
N/A
Reflow resistance
240°C peak temperature, 4 times
Pass
N/A
leads/in2 (2,753 leads/cm2).28 At the same time, flip chip packages are increasingly being made from laminate materials instead of the more conventional ceramic or thin-film technologies. To meet these needs, a new generation of printed circuit boards and laminate packages is needed that can achieve the high density required. The density in conventional substrate technology is primarily limited by the need to drill through the entire stack to achieve vertical interconnections. Large capture pads are required and, in the layers where the connection is not desired, circuitry must be routed around these drilled vertical interconnects. To achieve blind and buried vias using printed circuit board technology, one approach is to use controlled-depth drilling. TABLE 7.8
Reliability Test Results for ALIVH-B
Test description
Test conditions
Results
High-temperature storage
150°C, 2000 h
Pass
Low-temperature storage
−65°C, 2000 h
Pass
High-temperature and highhumidity storage
85°C/85% RH, 2000 h
Pass
Pressure cooker test (PCT)
121°C, 0.2 MPa, 200 h
Pass
Thermal shock (high and low temperature)
−65°C for 30 min to 150°C for 30 min, 1000 cycles
Pass
Thermal shock (high-temperature immersion)
20°C for 10 s to 260°C for 10 s, 200 cycles
Pass
Reflow soldering heat
260°C for 10 s, 10 cycles
Pass
High temperature and humidity + reflow heat
85°C/85% RH, 16 h + 260°C, 10 s, 3 times
Pass
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
237
However, mechanical drilling depth control is limited to ⫾35µm. Alternatively, sequential lamination of predrilled copper-clad laminate sheets and prepregs has also been used to make blind and buried via constructions. Ultimately, however, these approaches are limited not only by the capabilities of the mechanical drilling to make the fine vias, but also by their high cost. Drilling costs increase substantially for smaller holes, with the cost for 100-µm (4 mil) holes being 18 times that for 340-µm (13.5 mil) holes.29 Furthermore, capture pads still remain an issue with this approach. A number of novel blind and buried via technologies have been proposed over the last few years to eliminate the density limitation. Most of these techniques utilize additive or sequential build-up. Because of this, and because of the fact that the vias are small compared to standard drilled vias, these structures are alternately called build-up technologies (BUT) or microvia technologies. They are generally classified according to the different methods of via formation as photovia, plasmaetched via, and laser-drilled via technologies. The first of these uses permanent photoimageable inner-layer dielectric materials (coated liquids or laminated dry films) that are photoprocessed similarly to solder mask materials, except that these materials are designed to remain on the board permanently and become the inner layers. Plasma processing, the second of these, utilizes plasma ablation of dielectric, most commonly using the top copper circuit as an etch mask. The last technique, laser drilling, is done by ablation of the via using a conformal mask or a directly focused beam, with either a UV-Nd:YAG or a CO2 laser. Combinations of the laminate technology with thin-film deposition have also shown good results, but carry a substantial penalty in capital equipment costs. An alternative approach that addresses both the in-plane and vertical density requirements as well as price targets uses circuit “layer pairs” manufactured using adhesiveless copper clad polyimide film. Roll-to-roll manufacturing allows cost reduction through reduced labor costs and improved yields.30 Prior to deposition of any metal, 1- to 2-mil vias are laser-cut into the unreinforced, precast polyimide film in a regular grid pattern or in specified locations. The planar surfaces and vias are then simultaneously metallized, resulting in a significant cost savings in processing. High-density layer pairs with virtually landless through-holes can thus be constructed on a very cost-effective basis. These layer pairs can be laminated to create a multilayer circuit using conventional drilled stack vertical interconnection. Traditionally, vertical interconnection in these multilayer stacks is accomplished by drilling and plating holes through the entire construct. An innovative interconnection strategy is required to reclaim the wasted real estate
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
238
Chapter Seven
on both surface and interior layers that is endemic to this process. However, in order to take the best advantage of the technology, blind and buried vertical interconnections are required on a layer-to-layer basis. One method of achieving cost-effective selective interconnection uses an anisotropically conductive adhesive film. While this approach supports the creation of low- and medium-density vertical interconnects, it is not capable of achieving higher densities and does not adequately address the issue of dielectric separation between layers. The alternative approach presented here uses a patterned organic-metallic TLPS conductive composite material to achieve a high-density, reliable vertical interconnect. 7.4.1 TLPS conductive composite
Most conductive polymer materials are thermosetting or thermoplastic resins loaded with metal powder that provides conduction through contact of particles. They can be either isotropic or anisotropic depending on the level of the conductive particle loading and the method of application. The main deficiencies of these passively loaded polymers occur with temperature and humidity fluctuations. These fluctuations cause loss of electrical continuity due to the oxidation of the contact pads and the expansion of the polymer.31 In addition, no metallurgical connection is formed with the pads when conventional conductive compositions are used. These deficiencies are addressed by a novel conductive composite material that was introduced a few years ago for the purpose of replacing copper traces in selected applications.32 The combination of TLPS of the metals and a permanent adhesive flux binder delivers electrical conduction through sintered metal joints and mechanical properties based on a tailorable polymer matrix. In some ways, these materials are analogous to cermets, except that unlike the ceramic composites, processing of Ormet® (organic-metallic) composites is done at temperatures compatible with standard printed circuit board materials and processing conditions. Once cured, the material is stable in thermal exposures well above the initial process temperature. These conductive composites overcome several of the disadvantages of passively loaded compositions. Of particular importance to the application for vertical interconnection, they provide a low and stable bulk resistance value on the order of 35 µΩ/cm. This stable electrical performance under both normal use and environmental and thermal cycling is the result of the alloyed metallurgical web. This alloyed web microstructure is contiguous not only through the bulk material, but to solderable pad finishes as well.
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
239
Specialized versions of these TLPS conductive composites have been used in applications as diverse as fabrication of additively processed circuit boards with fine lines and blind and buried microvias, surface mount attach of electronic components, and vertical interconnections for the fabrication of the high-density substrates presented here. In the development of TLPS composite materials for the vertical interconnect application, the following parameters were considered: interconnect configuration used, application methodology, B-staging conditions and requirements, and lamination/joining conditions. With these issues in mind, appropriate TLPS composites were developed for the two primary methods of vertical interconnect investigated and described here. 7.4.2 High-density multilayer substrate development33–38
Development of vertical interconnections was undertaken in conjunction with the development of multilayer lamination. This included consideration of a number of issues including feature sizes, type of adhesive system, vertical interconnect configuration, application methodologies for the Ormet® composite material, and lamination conditions. Double-sided circuits (layer pairs) were first constructed of polyimide with drilled and plated vias and copper circuits. Initial circuit features were 50-µm (2 mil) lines and spaces and 200-µm (8 mil) pads on 500-µm (20 mil) pitch. A micromachining laser was used to drill vias in specified locations in the film that were then plated up. Vias in the layer pairs were typically 25 µm (1 mil). Later work used 38-µm (1.5 mil) lines with 50-µm spaces and 125-µm (5 mil) pads. These layer pairs were then laminated using various B-stage adhesive systems. Vertical interconnections were established in a number of configurations that utilized the TLPS conductive composite. A significant amount of the development was devoted to choosing the appropriate B-stage adhesive system for the construction. Reinforced and nonreinforced adhesives were examined. Issues of importance included thermal, dimensional, and mechanical material properties, handling, lamination at close to standard printed circuit board industry temperatures, flow of the adhesive system, circuit and interconnect encapsulation, and dielectric separation control. Among the reinforced systems, both woven and nonwoven fiber reinforcements were examined for their properties with regard to drilling capabilities and resin flow during lamination. Nonreinforced systems explored included glasssphere-filled adhesives as well as adhesives coated on polyimide film. While the former has shown promise and will be important as the
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
240
Chapter Seven
dimensions get finer, the adhesive materials used in the constructions discussed here were of the reinforced type or coated on film. 7.4.3 Vertical interconnect configurations
The three basic vertical interconnect configurations developed are shown in Fig. 7.28. The first of these uses a perforated B-stage dielectric bond-ply material. The vias in the bond-ply are filled with the TLPS composite by one of many methods including stenciling, doctor blading with the use of a cover sheet, or filling the pattern-perforated dielectric with a custom pressure-assisted tool. The bond-ply is then placed between the two parts that are to be connected, aligned, and cured. The second configuration uses stenciling of the TLPS composite directly onto the circuit pads of the top layer to create a post. The post serves as a contact point and is aligned with a copper pad on the circuit that is to be connected. The composite will form a metallurgical bond with both pads during the cure cycle. In both configurations, the vertical interconnection relies totally on the Ormet® conductive composite to achieve the vertical interconnect link (OrmeLink). The third configuration uses stenciling of the TLPS composite directly onto the circuit pads of the top layer, but this time it is used to
Three configurations of vertical interconnects utilizing TLPS conductive composite.
Figure 7.28
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
241
create a reduced-volume post. The bottom layer is plated up with a copper post. When the two layers are aligned, the plated post will make contact with the B-staged TLPS ink post and in the lamination cycle a metallurgical connection will be made between the two posts. This configuration relies on the combination of post and TLPS composite to achieve the vertical interconnect. In all cases, the TLPS material is B-staged for handling and storage life. The circuit layer pairs and the bond-ply sheets are interleaved and aligned and the stack is inserted into a lamination press. Lamination conditions are typical of printed circuit board industry practices. A variety of test structures have been used to determine the properties of vertical interconnects using TLPS composites. Early work highlighted the importance of concurrent engineering in the choice of materials and process conditions. Following the feasibility experiments, two representative test vehicles were developed using the structures described previously. The first was a six-layer structure that is being developed as a flip chip substrate. This structure used configuration I or III. The second was a selective multilayer patch for high density in certain portions of the circuit board. It used the TLPS contact points described in configuration II. 7.4.4 Multilayer chip package
As mentioned before, flip chip package substrates require high densities in order to route the signal from the die. Increased I/O means finer lines and spaces as well as smaller pads and vias. This also requires the capability of stacking the vias in the substrate. A six-layer daisy chain test vehicle designed to emulate a multilayer flip chip package was used to develop the methods for achieving vertical interconnections using the TLPS conductive composites. The structure used 200-µm-diameter pads, which is adequate for a 500- to 700-pin package. Figure 7.29 shows the cross-section of a six-layer structure in which the adhesivecoated 50-µm polyimide film was filled with the TLPS conductive composite and laminated between two pads. The alignment of the vertical stack is within ⫾12 µm. For 1600-pin packages, 125-µm or smaller pads will be required. Development is currently under way on both of the previously mentioned vertical interconnect configurations to achieve these higher densities. Figure 7.30 shows a cross section of stacked vias made using the method of plated posts and reduced-volume TLPS posts to connect two 100-µm pads. The plated posts are connected to the TLPS posts as seen in Fig. 7.30. Vias of this size have been used to connect 200-µm pads, but smaller pads are possible, although registration may be an issue. Smaller vias are also considered feasible with this approach. The lim-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
242
Chapter Seven
Figure 7.29
Cross section of vertical interconnects between 200-µm pads in a multilayer
substrate.
its of this technology have also been under investigation. Figure 7.31 shows the 225-µm pads connected with 55-µm TLPS joints in an eightlayer structure. In this case the whole joint is made of the composite material. Even though the pads in this case were rather large, the cross-section reveals that with proper registration, pad size could be significantly reduced. 7.4.5 Selective multilayer patch
Many applications, such as those required for flip chip attach, require high densities only in certain areas of the board. In these situations, it is uneconomical to fabricate the entire printed circuit board at this high density level. To overcome this problem, a layer pair patch can be laminated onto a conventionally fabricated low-density printed circuit board to create a localized area of high density. This concept is illustrated in Fig. 7.32. The electrically conductive adhesive contact points illustrated in Fig. 7.32 were created by stencil printing on top of plated posts. This approach (configuration II) was used because of the availability of large interconnection pads on the low-density PCB. Additionally, the printed circuit board used in this case had a through-hole to which this patch was connected, thus necessitating a larger post to achieve the
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
Figure 7.30
243
Cross section of stacked plated post/TLPS composite vias between 100-µm
pads.
Cross section of an eight-layer circuit that uses conductive composite-filled bond-ply.
Figure 7.31
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
244
Chapter Seven
Figure 7.32
High-density laminate patch application.
vertical connection. A top view of the laminated PCB with the highdensity patch underneath is given in Fig. 7.33. A cross section of the vertical connection between the TLPS conductive composite stenciled on a plated post and a 0.5-mm (20 mil) plated through-hole on a low-density PCB is seen in Fig. 7.34. The TLPS conductive composite forms a metallurgical contact with the copper (blind joint on the side of the through-hole) and also fills part of the throughhole in the low-density PCB, forming a good fillet. This construction was then laminated to a heat sink as shown in Fig. 7.32 and subsequently assembled with components. This product is currently undergoing long-term reliability testing in an automotive environment. The multilayer patch can also be applied on or incorporated between two or more standard PCBs. This design allows for the construction of a multilayer structure with the use of standard printed circuit boards.
High-density film patch laminated onto a lowdensity PCB.
Figure 7.33
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
Conductive Paste/Ink-Filled Microvias
245
Figure 7.34 Cross section of a vertical interconnect made for a high-density patch.
7.4.6 Reliability test results
The constructions discussed have been tested for shorts and opens. Some of them have also been subjected to basic reliability testing. Multilayer connections with 200-µm pads that use the plated post and the TLPS post approach have been tested with 250 liquid-to-liquid thermal shocks (−100 and +100°C, 3 min at each extreme with 15-s transfer). After every 25 cycles, measurements were taken to determine the resistance of each daisy chain pattern, which includes 1857 25-µm plated copper vias and 1238 100-µm post joints. There were no failures in the seven daisy chain samples tested, and the change in resistance averaged less than 10 percent. Constructions that used an all-TLPS joint were also subjected to environmental testing. Humidity testing at 85°C/85 RH for 7 days as well as 1000 air-to-air thermal shock cycles between −55 and +150°C showed less than 10 percent change in resistance. The all-TLPS joints averaged less than 10 mΩ, with most being less than 5 mΩ. With the drive toward higher density substrates, laser processing has allowed the fabrication of a circuit layer pair with plated vias as small as 25 µm. To achieve a high-density multilayer construction, lamination of the layer pairs is needed with appropriate vertical interconnects. Several approaches have been explored for this purpose, including various anisotropic adhesives. As an alternative, the use of patterned TLPS vertical interconnects guarantees a better electrical connection as well as assurance of controlled dielectric separation with the use of an appropriate bond-ply. The TLPS conductive composites used for vertical interconnects either alone or in combination with a plated post have demonstrated the capability of joining pads as small as 100 µm to create multilayer structures. The composites form a good metallurgical connection to the circuit pads, as shown by the cross sec-
Downloaded from Digital Engineering Library @ McGraw-Hill (www.digitalengineeringlibrary.com) Copyright © 2004 The McGraw-Hill Companies. All rights reserved. Any use is subject to the Terms of Use as given at the website.
Conductive Paste/Ink-Filled Microvias
246
Chapter Seven
tions of the eight-layer circuits done so far. These composites are currently being tested for multilayer chip carriers as well as for attachment of high-density multilayer circuit patches. Environmental and electrical testing is under way at several companies. The substrates that are feasible with the use of these technologies offer a number of advantages over current interconnect densities. The fine-line capabilities of the flexible circuit layer pairs together with the very fine vias in the layer pairs and in the bond-ply allow for very dense circuitry in a thin substrate. Additionally, this technology allows for buried, blind, and stacked vias, which will further enhance the circuit density and allow for reduction of the layer count. 7.5 References 1. Lau, J. H., and C. Chang, “An Overview of Microvia Technology,” Circuit World, 26(2): 22–32, January 2000. 2. Boggio, B., “The Any-Layer Interstitial Via Hole Processes,” Board Authority, 2(1): 91–95, April 2000. 3. Matijasevic, G., C. Gallagher, and P. Gandhi, “High Density Multilayer Substrates Using Patterned Microvia Interposers,” Proceedings of IEEE Aerospace Conference, Snowmass, CO, March 1998. 4. Kang, S. K., S. Buchwalter, N. LaBianca, J. Gelorme, and S. Purushothaman, “Development of Conductive Adhesive Materials for Via Fill Applications,” Proceedings of 50th ECTC Conference, pp. 887–991, Las Vegas, NV, May 2000. 5. Gilleo, K., “Die Attachment for Today’s Packaging Challenges,” Elec. Pack. Prod., 2: 109, 1994. 6. Gilleo, K., “Evaluating Polymer Solders for Pb-Free Assembly,” Circuit Assembly, 1: 52, 1994. 7. Saraf, R. F., and J. M. Roldan, “Polymer/Metal Composite for Interconnection Technology,” Proceedings of 45th Elec. Comp. Tech. Conf., p. 1051, Las Vegas, NV, 1995. 8. Gallagher, C., G. Matijasevic, and M. Capote, “Transient Liquid Phase Sintering Conductive Adhesives,” Proceedings of Surf. Mount Tech. Int. Conf., p. 568, San