Studies in Surface Science and Catalysis 97 ZEOLITES: A REFINED TOOL FOR DESIGNING CATALYTIC SITES
This page intentionally left blank
Studies in Surface Science and Catalysis Advisory Editors: B. Delmon and J.T. Yates Vol. 97
ZEOLITES: A REFINED TOOL FOR DESIGNING CATALYTIC SITES Proceedings of t h e International Zeolite S y m p o s i u m , Qu(~bec, O c t o b e r 15-20,1995
Canada,
Edited by
Laurent Bonneviot Departement de Chimie, CERPIC, Facu/te des Sciences et de Genie, Universite Lava/, Quebec, Canada G 1K 7P4
Serge Kaliaguine Departement de Genie Chimique, CERPIC, Faculte des Sciences et de Genie, Universite Lava/, Quebec, Canada G 1K 7P4
1995 ELSEVIER A m s t e r d a m - - L a u s a n n e - - N e w Y o r k - - O x f o r d --- S h a n n o n --- T o k y o
ELSEVIER SCIENCE B.V. Sara Burgerhartstraat 25 P.O. Box 521, 1000 AM Amsterdam, The Netherlands
ISBN 0-444-82130-9 91995 Elsevier Science B.V. All rights reserved. No part of this publication may be reproduced, stored in a retrieval system or transmitted in any form or by any means, electronic, mechanical, photocopying, recording or otherwise, without the prior written permission of the publisher, Elsevier Science B.V., Copyright & Permissions Department, P.O. Box 521, 1000 AM Amsterdam, The Netherlands. Special regulations for readers in the U.S.A.- This publication has been registered with the Copyright Clearance Center Inc. (CCC), 222 Rosewood Drive, Danvers, MA 01923. Information can be obtained from the CCC about conditions under which photocopies of parts of this publication may be made in the U.S.A. All other copyright questions, including photocopying outside of the U.S.A., should be referred to the copyright owner, Elsevier Science B.V., unless otherwise specified. No responsibility is assumed by the publisher for any injury and/or damage to persons or property as a matter of products liability, negligence or otherwise, or from any use or operation of any methods, products, instructions or ideas contained in the material herein. This book is printed on acid-free paper. Printed in The Netherlands
CONTENTS Foreword . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Acknowledgements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . PL-1
M-l-1
One and Two-Dimensional Solid-State NMR Investigations of the ThreeDimensional Structures of Zeolite-Organic Sorbate Complexes C.A. Fyfe, H. Grondey, A.C. Diaz, G.T. Kokotailo, Y. Feng, Y. Huang, K.C. Wong-Moon, K.T. Mueller, H. Strobl and A.R. Lewis . . . . . . . . . . . . .
XI XII
1
The Use of Small, Weakly Basic Probe Molecules for the Investigation of BrCnsted Acid Sites in Zeolites by NMR Spectroscopy E. Brunner . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
11
Determination of the Environment of Titanium Atoms in TS-1 Silicalite by Ti K-edge X-ray Absorption Spectroscopy, 29Si and 1H Nuclear Magnetic Resonance- L. Le Noc, C. Cartier dit Moulin, S. Solomykina, D. Trong On, C. Lortie, S. Lessard and L. Bonneviot . . . . . . . . . . . . . . . .
19
An in situ 13C MAS NMR Study of Toluene Alkylation with Methanol over H-ZSM-11 - I.I. Ivanova and A. Corma . . . . . . . . . . . . . . . . . . . . . .
27
KL-1
Strategies for Zeolite Synthesis by Design- M.E. Davis . . . . . . . . . . . . . .
35
M-2-1
Use of Modified Zeolites as Reagents Influencing Nucleation in Zeolite Synthesis - S.I. Zones and Y. Nakagawa . . . . . . . . . . . . . . . . . . . . . . . . .
45
Templating Studies Using 3,7-Diazabicyclo[3.3.1]nonane Derivatives: Discovery of New Large-Pore Zeolite SSZ-35 - Y. Nakagawa . . . . . . . . . .
53
Synthesis of ZSM-48 Type Zeolite in Presence of Li, Na, K, Rb and Cs Cations - G. Giordano, A. Katovic, A. Fonseca and J.B. Nagy
61
Out-of-Plane Bending Vibrations of Bridging OH Groups in Zeolites: A New Characteristic of the Geometry and Acidity of a Broensted Site - L.M. Kustov, E. Loeffler, V.L. Zholobenko and V.B. Kazansky
63
In situ FTIR Microscopic Investigations on Acid Sites in Cloverite G. MUller, G. Eder-Mirth and J.A. Lercher . . . . . . . . . . . . . . . . . . . . . . .
71
Broensted Sites of Enhanced Acidity in Zeolites: Experimental Modelling - M.A. Makarova, S.P. Bates and J. Dwyer . . . . . . . . . . . . . . . .
79
Modelling of Structure and Reactivity in Zeolites - C.R.A. Catlow, R.G. Bell, J.D. Gale and D.W. Lewis . . . . . . . . . . . . . . . . . . . . . . . . . . .
87
M-l-3
M-l-4
M-2-2
M-2-3
M-2-4
M-2-5
M-2-6
PL-2
VI
Tu-l-1
Tu-l-2
Tu-l-3
Tu-l-4
KL-2
Tu-2-1
Tu-2-2
Tu-2-3
Tu-2-4
Tu-2-5
Computational Studies of Water Adsorption in Zeolites - S.A. Zygmunt, L.A. Curtiss and L.E. Iton . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
101
Modeling of Adsorption Properties of Zeolites - A. Goursot, I. Papai, V. Vasilyev and F. Fajula . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
109
Loading and Location of Water Molecules in the Zeolite Clinoptilolite Y.M. Channon, C.R.A. Catlow, R.A. Jackson and S.L. Owens . . . . . . . . . .
117
Withdrawal of Electron Density by Cations from Framework Aluminum in Y-Zeolite Determined by A1 XAFS Spectroscopy D.C. Koningsberger and J.T. Miller . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
125
Geometry of the Active Sites in Zeolites under Working Conditions F. Fajula . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
133
Characterization of Hexagonal and Lamellar Mesoporous Silicas, Alumino- and Gallosilicates by Small-Angle X-Ray Scattering (SAXS) and Multinuclear Solid State NMR - Z. Gabelica, J.-M. Clacens, R. Sobry and G. Van den Bossche . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
143
Characterization of a Cubic Mesoporous MCM-48 Compared to a Hexagonal MCM-41 - R. Schmidt, M. St6cker and O.H. Ellestad . . . . . . . .
149
Synthesis and Characterization of Transition Metal Containing Mesoporous Silicas - S. Gontier and A. Tuel . . . . . . . . . . . . . . . . . . . . . .
157
Bimodal Porous Materials with Superior Adsorption Properties C.J. Guo . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
165
MCM-41 Type Silicas as Supports for Immobilized Catalysts - D. Brunel, A. Cauvel, F. Fajula and F. DiRenzo . . . . . . . . . . . . . . . . . . . . . . . . . . . .
173
Tu-2-6
Synthesis of Mesop0rous Manganosilicates Mn-MCM-41, Mn-MCM-48 and Mn-MCM-L at a Low Surfactant/Si Ratio - D. Zhao and D. G o l d f a r b . . 181
W-l-1
Alkane Oxidation Catalyzed by Zeolite Encapsulated Ruthenium Perfluorophthalocyanines - K.J. Balkus Jr., A. Khanmamedova and M. Eissa . . . . . .
189
W-l-2
MOCVD in Zeolites Using Mo(CO) 6 and W(CO)6 as Precursors - S. Djajanti and R.F. Howe . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 197
W-l-3
Tailored Synthesis, Characterization and Properties of ZnO, CdO and SnO 2 Nano Particles in Zeolitic Hosts - M. Wark, H.-J. Schwenn, M. Warnken, N.I. Jaeger and B. Boddenberg . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
205
VII
Host-Guest Interactions in Zeolite Cavities - A. Zecchina, R. Buzzoni, S. Bordiga, F. Geobaldo, D. Scarano, G. Ricchiardi and G. Spoto . . . . . . . .
213
PL-4
Diffusion in Zeolites - D.M. Ruthven
223
Th-l-1
Frequency Response Study of Mixture Diffusion of Benzene and Xylene Isomers in Silicalite-1 - D. Shen and L.V. Rees . . . . . . . . . . . . . . . . . . . .
235
2D EXSY 129Xe NMR: New Possibilities for the Study of Structure and Diffusion in Microporous Solids - I.L. Moudrakovski, C.I. Ratcliffe and J. Ripmeester . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
243
Diffusion of C10-C24n-paraffins and perfluorotributylamine in clay catalysts- B. Liao, M. Eic, D.M. Ruthven and M.L. Occelli . . . . . . . . . . .
251
Sorption Properties of Dealuminated Large Crystals of ZSM-5: A New Approach to the Description of Isotherms- J. Kornatowski, M. Rozwadowski, W. Lutz and W.H. Baur . . . . . . . . . . . . . . . . . . . . . . .
259
Convective Methods to Investigate Multi-component Sorption Kinetics on Microporous Solids- A. Micke and M. Btilow . . . . . . . . . . . . . . . . . . .
269
KL-4
Zeolites as the Key Matrix for Superior deNOx Catalysts - T. Inui . . . . . . .
277
Th-2-1
Catalytic Properties of Palladium Exchanged Zeolites in the Reduction of Nitrogen Oxide by Methane in the Presence of Oxygen: Influence of Hydrothermal Ageing - C. Descorme, P. G61in, M. Primet, C. L6cuyer and J. Saint-Just . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
287
The Effect of Preparation and Steaming on the Catalytic Properties of Cu- and Co-ZSM-5 in Lean NO x Reduction - P. Ciambelli, P. Corbo, M. Gambino, F. Migliardini, G. Minelli, G. Moretti and P. Porta . . . . . . . .
295
Adsorption Sites for Benzene in the 12R Window Zeolites: A Molecular Recognition Effect- B.L. Su . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
303
Lewis Basic and Lewis Acidic Sites in Zeolites - M. Huang, S. Kaliaguine and A. Auroux . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
311
Effect of the Framework Composition on the Nature and the Basicity of Intrazeolitic Cesium Oxides. Correlation Activity/Basicity - M. Lasp6ras, I. Rodriguez, D. Brunel, H. Cambon and P. Geneste . . . . . . . . . . . . . . . . .
319
KL-3
Th-l-2
Th-l-3
Th-l-4
Th-l-5
Th-2-2
Th-2-3
Th-2-4
Th-2-5
...........................
VIII Th-2-6
F-l-1
F-l-2
F-l-3
F-l-4
KL-5
F-2-1
F-2-2
F-2-3
F-2-4
P-2
P-6
Hydrothermal and Alkaline Stability of High-Silica Y Zeolites Generated by Combining Substitution and Steaming - W. Lutz, E. LOftier and B. Zibrowius . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
327
Electron Spin Resonance and Electron Spin Echo Modulation Spectroscopy of Ni(I) in SAPO-5 and SAPO-11 - M. Hartmann, N. Azuma and L. Kevan . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
335
Selective Acidic, Oxidative and Reductive Reactions over ALPO-11 and Si or Metal Substituted ALPO-11 - P.S. Singh, R. Bandyopadhyay, R.A. Shaikh and B.S. Rao . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
343
Characterization and Catalytic Performance of PdSAPO-5 Molecular Sieves - T.-C. Xiao, L.-D. An and H.-L. Wang . . . . . . . . . . . . . . . . . . . . .
351
FTIR Study of the Acidic Properties of Substituted Aluminophosphates V. Zholobenko, A. Garforth, L. Clark and J. Dwyer . . . . . . . . . . . . . . . . .
359
Selective Oxidation with Redox Metallosilicates in the Production of Fine Chemicals- P. Ratnasamy and R. Kumar . . . . . . . . . . . . . . . . . . . . .
367
Novel Model Catalysts Containing Supported MFI-type Zeolites N. van der Puil, E.C. Rodenburg, H. van Bekkum and J.C. Jansen . . . . . . .
377
Oligomerization of Butenes with Partially Alkaline-Earth Exchanged NiNaY Zeolites - B. Nkosi, F.T.T. Ng and G.L. Rempel . . . . . . . . . . . . . .
385
Isomerization of C 8 Aromatic Cut. Improvement of the Selectivity of MOR- and MFI- Catalysts by Treatments with Aqueous Solutions of (NH4)2SiF6 - E. Benazzi, J.M. Silva, M.F. Ribeiro, F.R. Ribeiro and M. Guisnet . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
393
Contribution of Framework and Extra-framework A1 and Fe Cations in ZSM-5 to Disproportionation and C 3 Alkylation of Toluene - J. (2ejka, N. Zilkov~i, Z. Tvart)~kov~i and B. Wichterlov~i . . . . . . . . . . . . . . . . . . . . .
401
NO x Adsorption Complexes on Zeolites Containing Metal Cations and Strong Lewis Acid Sites and their Reactivity in CO and CH 4 Oxidation: a Spectroscopic Study - L.M. Kustov, E.V. Smekalina, E.B. Uvarova and V.B. Kazansky . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
409
Cracking of 1,3,5-triisopropylbenzene over Deeply Dealuminated Y Zeolites- E.F. Sousa-Aguiar, M.L. Murta VaUe, E.V. Sobrinho and D. Cardoso . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
417
IX
P-7
P-11
P-14
P-15
P-16
P-17
P-18
P-19
P-20
P-21
P-25
P-26
P-27
Hydrogenation of Styrene and Hydrogenolysis of 2-Phenylethanol T. Sooknoi and J. Dwyer . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
423
Catalyst Deactivation of High Silica Metallosilicates in Beckmann Rearrangement of Cyclohexanone Oxime - T. Takahashi, T. Kai and M.N.A. Nasution . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
431
IR Studies on the Reduction of Nitric Oxide with Ammonia over MFIFerrisilicate - T. Komatsu, Md. A. Uddin and T. Yashima . . . . . . . . . . . . .
437
The Role of the Na and of the Ti on the Synthesis of ETS-4 Molecular Sieve - P. De Luca, S. Kuznicki and A. Nastro . . . . . . . . . . . . . . . . . . . .
443
On the Potential of Zeolites to Catalyse the Aromatic Acylation with Carboxylic Acids - E.A. Gunnewegh, R. Downing and H. van Bekkum
447
Elimination of Methanol from Dimethylacetal over Aluminophosphate Molecular Sieves and Zeolites - S.-M. Yang and K.-J. Wang . . . . . . . . . . .
453
Deuteration of Zeolitic Hydroxyl Groups in the Presence of Platinum Evidence for a Spillover Reaction Pathway - U. Roland, R. Salzer and L. SUmmchen . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
459
IR Investigation of CO Adsorption at Low Temperature: A Key Tool to Characterize the Porosity of Matrix Embedded Zeolite Catalysts Z.M. Noronha, J.L.F. Monteiro and P. G61in . . . . . . . . . . . . . . . . . . . . . .
465
Identification of Active Ti Centers in TS-1 as Revealed by ESR Spectra of UV-Irradiated Samples - A. Ghorbel, A. Tuel, E. Jorda, Y. Ben TaCit and C. Naccache . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
471
Microwave Crystallization of Titanium-Containing Cloverite - R. Fricke, H.-L. Zubowa, J. Richter-Mendau, E. Schreier and U. Steinike . . . . . . . . . .
477
Aqueous Silicate Chemistry in Zeolite Synthesis - C.T.G. Knight, R.T. Syvitski and S.D. Kinrade . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
483
Effect of Hydrolysis Conditions of the Silicate Precursor on the Synthesis of Siliceous MCM-48 - J. Lujano, Y. Romero and J. Carrazza . . . . . . . . . .
489
Sorption of Light Alkanes on H-ZSM5 and H-Mordenite - F. Eder, M. Stockenhuber and J.A. Lercher . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
495
P-28
P-29
P-31
P-34
P-36
P-41
P-42
P-43
P-45
Acidity and Reactivity of Steamed HY Zeolites Obtained by Progressive Extraction of Extraframework A1 Species- L. Mariey, S. Khabtou, M. Marzin, J.C. Lavalley, A. Chambellan and T. Chevreau . . . . . . . . . . . .
501
L.
Adsorption of Nitrogen and Methane on Natural Clinoptilolite Predescu, F.H. Tezel and P. Stelmack . . . . . . . . . . . . . . . . . . . . . . . . .
507
Dealumination and Acidity Measurement of HEMT Zeolites Modified by Steaming and Leaching - O. Cairon, S. Sellem, C. Potvin, J.M. Manoli and T. Chevreau . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
513
The Synthesis of UTD-1, Ti-UTD-1 and Ti-UTD-8 Using CP*2CoOH as a Structure Directing Agent- K.J. Balkus Jr., A.G. Gabrielov and S.I. Zones . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
519
Zeolite Crystallization on Mullite Fibers - V. Valtchev, S. Mintova, B. Schoeman, L. Spasov and L. Konstantinov . . . . . . . . . . . . . . . . . . . . .
527
Synthesis and Characterization of V-Beta Zeolite - S.-H. Chien and J.-C. Ho . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
533
Titanium Boralites with MFI Structure Characterized Using XRD, IR, UV-Vis XANES and MAS-NMR Techniques - D. Trong On, M.P. Kapoor, S. Kaliaguine, L. Bonneviot and Z. Gabelica . . . . . . . . . . . .
535
Acidity and Structural State of Boron in Mesoporous Boron Silicate MCM-41 - D. Trong On, P.N. Joshi, G. Lemay and S. Kaliaguine . . . . . . .
543
The Role of Na and K on the Synthesis of Levyne-Type Zeolites C.V. Tuoto, J.B. Nagy and A. Nastro . . . . . . . . . . . . . . . . . . . . . . . . . . .
551
Author Index . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
557
Subject Index . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
561
Studies in Surface Science and Catalysis
567
................................
xI FOREWORD Once upon a time the catalytic use of zeolites was exclusively in the field of acid catalysis. Today zeolites also find applications as catalysts in a wide array of chemical reactions. These encompass base catalyzed reactions, Redox reactions and catalytic reactions on transition metals and their complexes in confined environments. The concepts of Bronsted or Lewis acid-base pairs are abundantly illustrated in the literature and better understood in terms of structural and electronic properties of zeolites. By contrast properties of chemically modified silicates, aluminosilicates and aluminophosphates are not yet fully explored. The list of oxydo-reduction reactions performed in the presence of these new materials is indeed continuously growing. For example the selective catalytic reduction of nitrogen oxides or the numerous oxidations employing hydrogen peroxide could be cited. In this context much effort is currently made in order to get a better insight into the nature of the sites involved. Thirdly, the zeolite lattice may be used as a host for encapsulated complexes or metallic clusters allowing to control the nuclearity of these active species and the steric constraints imposed on the reactants. The molecular sieve and shape selectivity effects have always constituted the most fascinating aspects of zeolite properties. The recent developments leading to increasingly large pore sizes with VPI-5, cloverite and more recently mesoporous molecular sieves have broadened the spectrum of these applications. Indeed larger and larger reactant and product molecules can be accommodated in these lattices. These new adsorbant/adsorbate systems create additional needs for experimental data and theoretical descriptions of transport properties, in particular of mono- and multicomponents diffusion coefficients in the zeolite pore lattice. All these questions represent the forefront and current trends of zeolite research. To various extends they deal with the specific factors of the zeolites which allow the fine tuning of the geometric and/or electronic properties of the active sites. It was indeed very rewarding for us, as organizers of this symposium, to realize that all these questions were actually discussed in the papers submitted to the selection committee and that they were widely represented in the selected papers. A feature general to most of these contributions is the combined use of a variety of analytical techniques. Some of these techniques are at the frontiers of the latest analytical developments such as multiple scattering EXAFS and bidimensional MAS-NMR. It is also worth mentioning that the on-going refinements of molecular modelling can now rely on more and more accurate quantum mechanics calculations such as the density functional theory (DFT) improved by introducing high level electron correlation. We wish to thank each and every one of the contributors to the Qu6bec International Zeolite Symposium, who gathered coming from not less than 27 countries to share their recent findings and ideas in a research field so liable to yield future fundamental developments as well as potential technical innovations.
Laurent Bonneviot and Serge Kaliaguine
XII PAPER SELECTION COMMITTEE
Y. BEN TA,M~T L. BONNEVIOT E.M. FLANIGEN Z. GABELICA M. GUISNET W.O. HAAG S. KALIAGUINE H.G. KARGE G.T. KOKOTAILO
L.B. McCUSKER W.J. MORTIER
J.M. NEWSAM T. TATSUMI H. van BEKKUM
Institut de Recherches sur la Catalyse, Villeurbanne, France Universit6 Laval, Qu6bec, Canada UOP, Tarrytown, NY, USA Facult6s Universitaires Notre-Dame de la Paix, Namur, Belgium Universit6 de Poitiers, Poitiers, France Mobil Research and Development Co., Princeton, NJ, USA Universit6 Laval, Qu6bec, Canada Fritz-Haber Institut der Max Planck, Gessleschaft, Berlin, Germany University of Pennsylvania, Philadelphia, PENN, USA and University of British Columbia, Vancouver, Canada Eidgentissische Technische Hochschule, Ztirich, Switzerland Exxon Chemical Europe Inc., Machelen, Belgium Biosym Technologies Inc., San Diego, CA, USA The University of Tokyo, Tokyo, Japan Delft University of Technology, Delft, The Netherlands
ACKNOWLEDGEMENTS
The organizers owe a huge debt of gratitude to Mrs. H61~ne Michel who contributed so efficiently to the Qu6bec Symposium organization as well as to the preparation of these proceedings.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
O n e and t w o - d i m e n s i o n a l solid-state N M R investigations of the threed i m e n s i o n a l structures of zeolite-organic sorbate c o m p l e x e s C.A. Fyfe, H. Grondey, A.C. Diaz, G.T. Kokotailo, Y. Feng, Y. Huang, K.C. Wong-Moon, K.T. Mueller, H. Strobl and A.R. Lewis Department of Chemistry, University of British Columbia, 2036 Main Mall, Vancouver, B.C. V6T 1Z1, Canada
1. I N T R O D U C T I O N A most important characteristic of molecular sieve systems which is common to their applications as catalysts, sorbents and in gas separation is the size and shape selectivity toward adsorbed organic molecules conferred by the molecular dimensions of their channel and cage systems [ 1]. Because of their small crystallite dimensions, powder rather than single-crystal XRD techniques must be used. While it is possible to define framework topologies and structures powder X-ray diffraction, particularly if Rietveld analysis and synchrotron radiation are used [2,3], it is very difficult to reliably determine the structures of organic sorbate/framework complexes which would yield important information on the detailed nature of the interactions. Important exceptions in this regard are the single crystal XRD studies of van Koningsveld and co-workers who determined detailed high-quality structures of the highloaded forms of p-xylene and p-dichlorobenzene in zeolite ZSM-5. These are the only reliable zeolite/sorbate structures to date [4,5]. High resolution solid state NMR has emerged in recent years as an important complementary technique to XRD in the investigation of zeolite structures, being particularly sensitive to short to medium range geometries and orderings [6]. For some years we have worked to develop new approaches in the application of solidstate NMR techniques together with XRD studies to the investigation of zeolite structures with the aim of ultimately being able to determine the 3D structures of their complexes with sorbed organic molecules. In this paper, we outline the development of these techniques and their current standing.
2. RESULTS AND DISCUSSION In high-resolution solid state NMR, the widths of the signals from dilute spin-1/2 nuclei are determined by the degree of crystallinity and the perfection of the local ordering. This can be achieved in the case of zeolites by investigating high-quality, completely siliceous systems where there is only the Si(4Si) local environment present. As illustrated in Figures 1A and B for ZSM-12 [7] and ZSM-5 [8], respectively, sharp resonances are observed whose numbers and relative intensities reflect the number and occupancy of the crystallographically inequivalent T-sites in the unit cell. In the case of A1PO4 molecular sieves, there is exact alternation of A1 and P, giving completely and perfectly ordered frameworks in the as-synthesized materials, as shown in Figure 1C for the 31p spectrum of VPI-5 [9]. This result is quite general for perfectly
crystalline and ordered solids. These spectra may be used to monitor various structural transformations, for example, those induced by temperature as in the case of ZSM-5 [ 10], or in the case of A1PO4 materials by the hydration/dehydration of octahedral A1 sites. Of particular importance, they yield information on the interaction of organic sorbates with the molecular sieve framework. For example, Figure 2 shows the 29Si spectrum of ZSM-5 with p-xylene present at a loading of two
A
I
I
I
-107
I
I
I
I
PPM from TMS
-113
A
Cl
0 I
I
I
I
-108
I
I
I
I
I
I
B
c~
C
,r
I
-118
PPM from TMS
C
J
I
25
~
I
0 Frequency
A
I
-25
.JO
-75
(ppm from 83% H3PO4)
Figure 1. 29Si MAS spectra of (A) ZSM-12 and (B) ZSM-5. (C) 31p MAS spectrum of VPI-5 with spinning sidebands indicated by brackets.
--I
-105
!
I
I
I
I
I
I
I
PPM / TMS
I
I
I
I
I
-120
Figure 2. 29Si MAS spectra of ZSM-5 loaded with 2 molecules per u.c. of (A) p-dichlorobenzene, (B) p-chlorotoluene, and (C) p-xylene.
molecules per unit cell (u.c.). Comparison with Figure 1B shows that the number of T-sites has decreased from 24 to 12 indicating a change in symmetry from monoclinic to orthorhombic. Further, the similarities between the spectra in the presence of p-xylene and pdichlorobenzene and p-chlorotoluene (Figure 2) indicate that the interactions, at least in this case, are based on the size and shape of the organic molecule since the CH3 and C1 substituents have the same steric factors but the molecules differ in most other aspects [ 11]. The difficulty in using these spectra further is that the assignment of the resonances to the different T-sites is generally not known, although there may be some information from the intensities if the site occupancies are different. In the case of ZSM-12 and ZSM-5, all of the site occupancies are the same and no assignments are possible. This problem can be solved by using two dimensional homonuclear correlation experiments such as COSY and INADEQUATE to establish the three-dimensional (Si-O-Si) connectivity pattern with the framework when the topology is known [12]. Figure 3 shows such an experiment on ZSM-12 [7]. This yields the assignments of the resonances shown in the figures. The above experiments are based on the scalar Si/Si J-coupling which operates through the bonding network. Similar information may be obtained in the A1PO4 systems from CP and TEDOR experiments as shown in Figure 4 [9]. Although these are based on the heteronuclear dipolar coupling which is a through-space interaction, they are selective for 3tp_ O-2VA1 connectivities because the interaction is very strongly distance dependent and these P/A1 distances are the shortest. Knowledge of the assignments may now be used to gain additional information on the details of the structures and the various changes which they can undergo. For example, zeolite ZSM- 11 is found to undergo a temperature induced transition from a
T3
T+ Ts
T1 T7
T5 T2
, ,
// /J
/
// T1T2 / / /
//
--T+T --.--,.~-.4.' ST // T3T5
0~,,
,/ T3TI
"~
,," T4T6 /
It
I
I
I
I
I
-108.0-109.0 -110.0 -111.0-112"0 -113.0
PPM Figure 3.
29Si INADEQUATE
experiment on ZSM-12.
i
1-------7----.-
I
I
I
I I I I I I I I I I
"
tr
O
o7 "
E o E
q tT.
I I
'
i, . . . . . . .
I
o
9
I
,
'10 Frequency
I
-20
,
I
-30
9
I
,
.40
I,
i_
-so
(ppm from 85% H3PO4)
Figure 4. Two-dimensional 27A1 ~ alp TEDOR experiment on VPI-5. The connectivities are displayed in the dashed box and spinning sidebands are indicated by asterisks. high-temperature form with seven T-sites which matches the proposed framework topology (tetragonal, space group I~,m2) to a lower symmetry form at room temperature (twelve T-sites with equal occupancy). 2D INADEQUATE experiments on both forms yield the assignments of the resonances shown in Figure 5 (see ref. [13] for more details) and from the relationship between the two spectra it can be deduced that the space group of the room temperature form is I4 (tetragonal) and that the phase transition involves the loss of the mirror plane. Information of this type is useful for further investigation of the structure by diffraction techniques. The last step in the extension of these solid state NMR techniques is to apply them to the investigation of the three dimensional structures of zeolite-sorbate complexes. This can be done by using experiments such as cross-polarization and REDOR which are based on the through-space dipolar interaction. Because of the strong distance dependence, the distances between the T-sites in the framework (whose identifies are now known) and nuclei on suitably isotopically substituted substrates may be determined, yielding the 3D structure of the zeolitesorbate complex. To test the validity of this approach we have investigated a number of such experiments applied to the high-loaded form of zeolite ZSM-5 containing p-xylene where the answer is known from the high-quality single crystal structure of van Koningsveld and coworkers [4].
A
I
B
T=302 K 133'
T=342 K
4Z
I
65
3 7
4
2 I
I
I
I
I
-110
I
PPM
2
I
I
I
I
- 118
I
I
I
I
I
- 109
PPM
2
I
I
I
I
-117
Figure 5. 29Si MAS spectra of ZSM- 11 at (A) 302 K and (B) 342 K. Below each spectrum is the deconvolution in terms of Lorentzian curves. In the present paper, the application of the CP technique with protons as the source nuclei will be described as representative of this class of experiments. In order to localize the polarization source as much as possible, experiments were carried out with the two specifically deuterated p-xylenes (1) and (2). CH 3
CD3
CH 3
CD3
(1)
(2)
D
D
Since the CP process is greatly dependent on molecular motions, these must be well understood for the system being studied. In the present work, these were investigated by wide line deuterium NMR of the sorbed organics. It was found that at 6 molecules/u.c., the methyl groups in the organic substrate have rapid C3v rotational motion while the aromatic rings are essentially rigid but a proportion show some low frequency "ring-flips" around the 1,4-axis. The effect of the distance dependence can be seen qualitatively from a comparison of the CP spectra with that from a simple one-pulse experiment as shown in Figure 6. The structure is orthorhombic with 24 T-sites of equal occupancy and the assignments of the resonances come as previously from 2D INADEQUATE experiments [14]. In the CP spectrum some signals are obviously enhanced compared to the others. The resonances due to the T-sites 1, 2, 10, 12 and 16 are quite well resolved and these were used in the study.
CP/MAS
MAS 13,Z314'6'8 I /I 20,~SlIznll
:"),2~ 19,9
7
18
I
I
'
I
-110
'
$
I
-112
'
I
12 1716
'
I
'
3 4
I
-114 -116 -118 PPM from TMS
'
I
"
I
-120
Figure 6. (a) 29Si CP/MAS spectrum of the complex of p-xylene (2) in ZSM-5 at a loading of 6 molecules per u.c. The contact time was 5 ms, with a recycle delay of 5 s. (b) 29Si MAS spectrum of the complex of p-xylene in ZSM-5 at a loading of 8 molecules per u.c. The spin-dynamics of the cross-polarization process from I to S nuclei as a function of time are described by Equation (1) [ 15]. S(t)
= Sma x (1 - Tcp/T1p(H)) -1
(exp(-t/Tlotn)) - exp(-t/Tcv))
(1)
Smax represents the theoretical maximum signal intensity obtainable from the polarization transfer, T1oca) the proton TIp value and Tcp the cross-polarization time constant. Thus the S signal intensity as a function of time should consist of an exponential growth controlled by the cross polarization transfer and an exponential decay due the T1o process. Of particular interest, Tcp can be related to the second moment of the IS dipolar interaction, (Ao~2)Is, as in Equation (2) and is proportional to rls6 as in Equation (3), [16]. 1
Tce
-
C (A(o 2 )IS
(2)
~ ( A('02 )II 2
1
Tcp
o~ (A002 )IS oc
2
7i~s E ris6
(3)
(a)
Si 12 x
12
--~--
Si 3 10 _..~tlB
Si 17
9
'si ~o-Si 1 Si12
" " ' I t .... ----D.--
8
Si17 Si 16
-"1"-. ---o--e
m
I
M
c o
Si 3
'
r&,
i
i
SI 16
qmo
Si 1
c
m
Si 10
O~ 0
10
20
30
Contact
(b)
40
time
50
60
(ms)
Si 1
1.2
Si 17 Si 10 1.0
A
=~--...._ m ~ ' m ~ ' " " . ~
=
Si 3 Si 16
r
. . ~ . . . . - . =. ~ t . ~ . . - 2 ~ ~ . . . .- .
0.8
I=
Si 12
>., i m
c o
0.6
"-=-"
:' F
C m
0.4
,S
/
. . . . x .... "'"Q""
0.2
-"-P-
e~
......s~ ~0
II
Si 1 Si 12
Si 17 Si~6
---=---si3 0.0
o
~o
2o Contact
so time
4o
so
eo
(ms)
Figure 7. Variation of the intensity as a function of the contact time for (a) the complex of pxylene (2) in ZSM-5 at a loading of 6 molecules per u.c., and (b) the complex of p-xylene (1) in ZSM-5 at a loading of 6 molecules per u.c.
Using these equations, the cross-polarization results can be related to the sorbate-lattice distances in the complex. Figure 7 shows the experimental CP curves for the well-resolved resonances of Figure 6 for complexes of p-xylenes (1) and (2) [17]. Qualitatively, it can be seen that silicons 12, 3 and 17 are much more efficiently polarized and hence closer to the ring protons than silicons 16, 10, 1 (Figure 7a), and that silicons 10, 1, 17 and 3 are closer to the methyl protons than silicons 16 and 12 (Figure 7b). More quantitatively, the data can be compared directly with the XRD data. The structure is found to have two sites, one at the channel intersections and one in the zig-zag channels (Figure 8), and the lattice sorbate distances and related second moments can be calculated. The CP curves in Figure 7 can be fitted by deriving the Tip(H) values from the clearest decays and using these data to deduce the Tcp values are shown in Table 1. Figure 9 shows the plot of the experimental Tcp values versus the calculated second moment values, validating the general approach used.
Si-2 Si-3
Si-4
Si-5 Si-13
Si-6
/ C
C~ C--
'
,.c
/
Si-17
,
rc
i
ic c
i '
/,, C C
I
I
CH3
Figure 8. View approximately along [001] of the single crystal structure of p-xylene in ZSM-5 at a loading of 8 molecules per u.c. Oxygen and hydrogen atoms are omitted for clarity.
(a)
(b)
180 T
450 T
160--
Sil0
Sil
4 0 0 - |-
140 -120 -"7
350 --
Si 17 Si3.
300 "7
100 -13. O
80--
~ 13. O
"
Si12
~ 12
~16
~
250
-
200
60 -
150
40-
100
| si 1/ t - / " s, ,6
" 0
~ 250
0 500
750
1000
Calc. second moment (Hz 2)
0
10000
I 20000
I 30000
Calc. second moment (Hz 2)
Figure 9. Plot of experimental Tcp values versus the calculated second moment (Ao32 )IS values for (a) the complex of p-xylene (2) in ZSM-5 at a loading of 6 molecules per u.c., and (b) the complex of p-xylene (1) in ZSM-5 at a loading of 6 molecules per u.c. Thus, in the one case where the structure is well described, the CP technique yields a result in good agreement with the known structure. Similar results have been obtained using the REDOR [18] technique. It is thus felt that with proper precautions and with particular attention to the motions of different parts of the organic guest molecules, solid-state NMR spectroscopy will be a viable technique for the determination of the structures of zeolite/sorbate complexes and that it will yield valuable complementary information to that from diffraction studies of these systems. It should be possible to combine the results from solid-state NMR with molecular dynamics calculations in an interactive manner.
3. A C K N O W L E D G E M E N T S C.A.F. acknowledges the support of the NSERC of Canada in the form of operating and equipment grants, Y.H. and K.T.M. for Postdoctoral Fellowships, and K.C.W-M. and
10 H.S. for Postgraduate Scholarships. A.C.D. thanks INTEVEP S.A. for a Postgraduate Scholarship. REFERENCES
1.
2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14.
15. 16. 17. 18.
(a) Meier, W.M. In Molecular Sieves. SCI Mong., 1968. (b) Breck, D.W. Zeolite Molecular Sieves; Wiley Interscience: New York, 1974. (c) Smith, J.V. Zeolite Chemistry and Catalysis; Rabo, J.A., Ed. ACS Monograph Series 171, American Chemical Society: Washington, DC, 1976. (d) Barrer, R.M. Zeolites and Clay Minerals as Sorbents and Molecular Sieves; Academic Press: London, 1978. W.I.F.; Harrison, W.T.A.; Johnson, M.W. High Resolution Powder Diffraction. Materials Science Forum; Catlow, C.R.A., Ed.; Trans Tech. Publication: Andermannsdorf, Switzerland, 1986; Vol. 9, pp. 89-101. The use of synchrotron x-ray sources may permit single crystal studies on much smaller samples. Eisenberger, P.; Newsam, J.B.; Leonowicz, M.E.; Vaughn, D.E.W. Nature, 1984, 309, 45. van Koningsveld, H.; Tuinstra, F.; van Bekkum, H.; Jansen, J.C. Acta Cryst., 1989, B45, 423. van Koningsveld, H.; Jansen, J.C. Private communication, to be published. Fyfe, C.A.; Gobbi, G.C.; Murphy, W.J.; Ozubko, R.S.; Slack, D.A.J. Am. Chem. Soc., 1984, 106, 4435. Fyfe, C.A.; Feng, Y.; Gies, H.; Grondey, H.; Kokotailo, G.T.J. Am. Chem. Soc., 1990, 112, 3264. Fyfe, C.A.; Strobl, H.; Kokotailo, G.T.; Kennedy, G.J.; Barlow, G.E.J. Am. Chem. Soc., 1988, 110, 3373. Fyfe, C.A.; Mueller, K.T.; Grondey, H.; Wong-Moon, K.C.J. Phys. Chem., 1993, 97, 13484. (a) Fyfe, C.A.; Kennedy, G.J.; Kokotailo, G.T.; Lyerla, J.R.; Fleming, W.W.J. Chem. Soc., Chem. Commun., 1985, 740. (b) Hay, D.G.; Jaeger, H.; West, G.W.J. Phys. Chem., 1985, 89, 1070. Fyfe, C.A.; Strobl, H.; Gies, H.; Kokotailo, G.T. Can. J. Chem., 1988, 66, 1942. Fyfe, C.A.; Feng, Y.; Grondey, H.; Kokotailo, G.T.; Gies, H. Chem. Rev., 1991, 91, 1525. Fyfe, C.A.; Feng, Y.; Grondey, H.; Kokotailo, G.T.; Mar, A. J. Phys. Chem., 1991, 95, 3747. (a) Fyfe, C.A.; Grondey, H.; Feng, Y.; Kokotailo, G.T.J. Am. Chem. Soc. 1990, 112, 8812. (b) Fyfe, C.A.; Grondey, H.; Feng, Y.; Kokotailo, G.T. Chem. Phys. Lett., 1990, 173, 211. (c) Fyfe, C.A.; Feng, Y.; Grondey, H.; Kokotailo, G.T.J. Chem. Soc., Chem. Commun., 1990, 1224. Mehring, M. Principles of High Resolution NMR in Solids. Second edition, 1983, Springer, Berlin. Pines, A.; Gibby, M.G.; Waugh, J.S.J. Chem. Phys., 1973, 59, 569. Fyfe, C.A.; Diaz, A.C.; Grondey, H.; Fahie, B. To be published. (a) Guillon, T.; Schaefer, J. J. Magn. Reson., 1989, 81,196. (b) GuiUon, T.; Schaefer, J. Adv. Magn. Reson., 1989, 13, 55.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviotand S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
11
The use of small and weakly basic probe molecules for the investigation of Bronsted acid sites in zeolites by N M R spectroscopy Eike Brunner Universit/it Leipzig, Fakult/it for Physik und Geowissenschaften, Linn6str~e 5, D-04103 Leipzig, Germany Small and weakly basic probe molecules were used for the characterization of Bronsted acid sites in zeolites by variable-temperature 1H and 13C NMR spectroscopy. It could be shown that the induced ~H NMR chemical shift A& of free surface hydroxyl groups caused by the adsorption of probe molecules as, e.g., CO and C2C14reflects the strength of acidity of the hydroxyls. The deprotonation energy AEDp of surface hydroxyl groups can be determined from A& if the influence of rapid thermal motions and/or exchange processes is suppressed. Furthermore, the use of the ~H NMR chemical shift &H..M of surface hydroxyl groups influenced by adsorbed probe molecules M as a sensitive qualitative measure for the strength of acidity is suggested. The geometry of the adsorption complexes formed by CO molecules hydrogen bonded to Bronsted acid sites could be determined by NMR spectroscopy.
1. INTRODUCTION The catalytic behaviour of H-zeolites with respect to Bronsted-acid catalyzed reactions is determined by the strength of acidity, the concentration, and the accessibility of the bridging hydroxyl groups which are known to act as Bronsted acid sites [1,2]. The strength of gas phase acidity of a surface hydroxyl group TO-H is defined as the inverse value of the Gibbs free energy change n GDp of the deprotonation
TO-H
~. T O -
+ H +
(1)
It could be shown [3] that AGDp is the sum of the deprotonation energy AEDp (heterolytic dissociation energy) and a constant contribution for surface hydroxyl groups in zeolites. Therefore, AEDpis a convenient measure for the strength of gas phase acidity. However, the spectroscopic measurement of the deprotonation energy ~EDp is still a subject of discussion. Both, IR and 1H MAS NMR spectroscopy allow the direct investigation of bridging hydroxyl groups (see, e.g., [1,2]). Very often the potential energy of the O-H stretching vibrations is approximated by the Morse potential. A dissociation energy Do can be calculated (see, e.g., [4,5]) from the wavenumbers Yon and v02 of the fundamental stretching vibration and the corresponding first overtone, respectively, according to
12
hcv oa Do ~"
(2)
4X
with
1 2YouZ = ~
V02
(3)
3VoH - v02
h denotes Planck's constant and c the speed of light in empty space. It has however been demonstrated by Kazansky [4,5] that Do is close to the value for the homolytic dissociation energy of the surface hydroxyl groups which strongly deviates from AEDp. Jacobs and Mortier [6,7] have found that VOH of free bridging hydroxyl groups (i.e., bridging hydroxyl groups which are not influenced by additional electrostatic interactions with the zeolite framework) correlates well with the intermediate Sanderson electronegativity. A corresponding correlation could also be found between the 'H NMR chemical shift ~H of free bridging hydroxyl groups and the intermediate Sanderson electronegativity. Therefore, Pfeifer et al. [1,8,9] have suggested to make use of 8H as a measure for the strength of acidity of free surface hydroxyl groups. This suggestion was confirmed by quantum chemical calculations [10] which have shown that AEDp and bn are linearly correlated for hydroxyl groups bound to T-atoms (B, A1, Si or P) whose first coordination sphere consists of oxygen atoms only. The slope of AEDp amounts to - 84 _ 12 kJ mol-' ppm -1. Since chemical shift differences can be measured with an experimental error of __+0.1 ppm it is possible to determine differences in the deprotonation energy of free surface hydroxyl groups with an accuracy of + 8 kJ mo1-1. Recent quantum chemical calculations [ 11] revealed that the deprotonation energy of terminal SiOH groups amounts to 1400 ___25 kJ mol-~ which excellently agrees with the experimentally determined value of 1390 kJ mol -~ [12]. Since the ~H NMR chemical shift of terminal SiOH groups amounts to 2.0 + 0.1 ppm the deprotonation energy AEDp can be calculated [13] according to
AF-,Dp -
kJmo1-1
1570-
84
8H
.
(4)
ppm
Paukshtis and Yurchenko [12,14] have developed another method for the determination of differences in the deprotonation energy of TO-H groups. This method is based on the measurement of the induced wavenumber shift Av = VOH...M - VOH, where VOH...Mdenotes the wavenumber of the stretching vibration of the surface hydroxyl groups influenced by adsorbed probe molecules M. Provided that (-Av) ~ 400 cm-' (weak hydrogen bonding) the deprotonation energy can be calculated according to the formula
13
A EDp
A ~ SiOH =
kJmo1-1
"-'~DP
_ 1
kdmo1-1
log
A
A._____~_v
(5)
A v s~on
with A = 0.00226 [12] and AEDpSiOH = 1400 kJ mo1-1 (see above). The deprotonation energy of different types of surface hydroxyl groups in zeolites was determined successfully by this method by the use of CO as the probe molecule M [15,16]. On the other hand, it is known that the formation of hydrogen bonds leads to a considerable broadening of the stretching vibration bands of surface hydroxyl groups. This leads to a relatively large experimental error for Av which limits the accuracy of the measurement especially of small differences in the deprotonation energy. It is known that the interaction between surface hydroxyl groups and adsorbed probe molecules M causes an induced 1H NMR chemical shift A8 = 8H..M - 8H, where 8H.M denotes the chemical shift of the surface hydroxyl groups influenced by the probe molecules. It could be shown [ 17] that ~H and VoH are linearly correlated at least in limited ranges. The slope of ~H amounts to 0.0147 ppm/cm-' for surface hydroxyl groups in zeolites and to 0.0092 ppm/cm-' for hydrogen bonded protons in various solids. It can therefore be supposed that the correlation between A b and (-A v) is given by
a8
ppm
_
(-av) -1
cm
(6)
with B-values between 0.0092 and 0.0147. If this is true it should be possible to make use of A ~ instead of Av in eq. (5).
2. EXPERIMENTAL NMR and diffuse reflectance FTIR measurements have been carried out on identical samples which were prepared in the following manner: Glass tubes were filled with the hydrated zeolite (bed depth: ca. 8 ram) and heated up to 673 K with a heating rate of 10 K/h under permanent evacuation. At this temperature the samples were further evacuated for 24 h at a final pressure of 10.2 Pa. Then the samples were cooled to 77 K and loaded with definite amounts of probe molecules (CO or C2C14). 13C enriched substances were used for the 13C NMR spectroscopic investigation of the adsorption state of the probe molecules. After loading the samples were sealed. NMR spectroscopic investigations have been carried out on a Bruker MSL 500 spectrometer at low temperatures since small probe molecules as CO can exhibit rapid thermal motions at room temperature. The lowest temperature achievable under magic angle spinning conditions in our laboratory yet amounts to 123 K. In contrast, static 13C NMR investigations were carried out at temperatures down to 4.5 K. All NMR chemical shifts are given relative to tetramethylsilane (TMS).
14 3. RESULTS AND DISCUSSION 3.1. General remarks The influence of small and weakly basic probe molecules on the low-temperature ~H MAS NMR spectra of zeolites was firstly investigated by White et al. [18]. Table 1 summarizes induced chemical shift values for a variety of probe molecules. Table 1 Induced ~H NMR chemical shift A8 of bridging hydroxyl groups in zeolite H-ZSM-5 loaded with different amounts of probe molecules M per framework A1 atom (A1F) measured at a temperature of 123 K. The data are taken from ref. [18]. probe molecule M
N2
CO
A 8/ppm (1 M/A1 F)
-
1.8
AS/ppm (2 M/A1 F)
0.3
1.8
C2H6
0.6
C2H4
C2H2
2.7
3.5
2.7
3.9
Convenient probe molecules should exhibit the following properties: (i) The induced 1H NMR chemical shift A8 caused by the probe molecules should be high since its relative experimental error is then low. (ii) A 8 should remain constant for coverages higher than 1 probe molecule per surface hydroxyl group. Otherwise the dependence of n 8 on the coverage has to be taken into account which complicates the use of A8 as a measure for the strength of acidity. (iii) The molecules must be chemically stable even in the presence of acid sites in zeolites. Conditions (i) and (ii) are obviously fulfilled for CO and C2H4. However, it turned out that C2H4 rapidly chemically reacts at room temperature in H-zeolites which makes its use as a probe molecule difficult. Therefore, CO and C2C14 (instead of C2H4) were chosen as promising candidates. 3.2. The interaction of CO molecules with bridging OH groups in zeolites The data collected in Table 2 (see next page) show that the induced 1H NMR chemical shift A8 caused by the interaction of surface hydroxyl groups in H-ZSM-5 with CO molecules qualitatively reflects the strength of acidity of the hydroxyls. However, it is doubtful that the induced chemical shift of bridging hydroxyl groups in the large cavities of zeolite 0.3 HNa-Y is smaller than that of the AIOH groups on non-framework A1 species in H-ZSM-5. Furthermore, the induced wavenumber shift of the free bridging hydroxyl groups in H-ZSM-5 amounts to ca. 330 cm -~ which is in good agreement with the results reported in refs. [15,19,20]. According to eq. (6) one would then expect an induced ~H NMR chemical shift of ca. 3.0 - 4.9 ppm which is in contradiction to the experimentally observed value of only 2 ppm. It could be shown that the CO molecules exchange rapidly between the bridging hydroxyl groups even at 123 K [18,21] and that the induced chemical shift A 8 has not reached its maximum value [22] which explains this contradiction. Rigid 13CO molecules should exhibit a broad signal with the typical shape of a line dominated by the chemical shift anisotropy. The principal values of the chemical shift tensor of rigid ~3COare 81~ = 822 = 8~ = 305 ppm and 8 3 3 = 81 ~---- - 48 ppm [23], i.e., the chemical
15 shift anisotropy amonts to Aoc = 353 ppm. The corresponding line shape could be found [24] for the 13C NMR signal of 13CO molecules physisorbed on silicalite measured at 4.5 K. Table 2 Experimental data for the ~H NMR chemical shifts 8i~ and 8H..CO as well as the induced chemical shift A8 of surface hydroxyl groups in zeolites. The measurements were carried out at 123 K. It should be mentioned that bridging hydroxyl groups influenced by an additional electrostatic interaction with the zeolite framework are not considered here. zeolite
hydroxyl group structure
H-ZSM-5 hydrothermally treated
0.3 HNa-Y
8H/ppm
bH...co/ppm
A8/ppm
SiOH
2.0
2.0
0.0
A1OH (on non-framework A1)
2.9
3.9
1.0
SiOHA1 (free)
4.2
6.2
2.0
SiOHAI (in the large cavities)
3.9
4.8
0.9
The 13C NMR spectrum of ~3CO molecules adsorbed on a zeolite H-Y measured at 123 K consists of a single narrow line at ca. 185 ppm indicating that the CO molecules still move isotropically. At a temperature of 4.5 K the spectrum exhibits a width corresponding to that expected for rigid 13CO molecules (see Fig. 1). It is important to mention that the transition from the narrow line observed for 123 K to the broad signal shown in Fig. 1 takes place at temperatures between 60 and 80 K. The 1H MAS NMR spectroscopic investigation of the interaction between surface hydroxyl groups and CO molecules should therefore be carried out at temperatures below 60 K which will be possible in the near future.
__...
S / ppm
[
I
600
400
r
l
200
r
I
0
I
-200
1
-400
Figure 1. 13C NMR spectrum of 13CO adsorbed on zeolite H-Y (Si/A1 = 2.5) measured at 4.5 K. The sample was loaded with ca. 26 molecules 13CO per unit cell.
16 It is remarkable that the characteristic line shape shown in Fig. 1 can only be observed for CO coverages which are not higher than the concentration of accessible bridging hydroxyl groups. It could be shown by IR spectroscopic investigations that all CO molecules are then adsorbed on bridging hydroxyl groups. The characteristic features of the spectrum shown in Fig. 1, namely the two maxima at the left edge of the spectrum and the "step" at the right edge vanish for coverages higher than the concentration of accessible bridging hydroxyl groups. In the latter case IR spectroscopic investigations reveal the existence of physisorbed CO besides CO molecules adsorbed on bridging hydroxyl groups. Therefore, it has to be concluded that the characteristic shape of the spectrum shown in Fig. 1 is not caused by a superposition of two different signals due to 13CO molecules in different adsorption states. It is known from IR spectroscopic investigations as well as quantum chemical calculations [25-27] that the adsorption of CO molecules on bridging hydroxyl groups leads to the formation of linear adsorption complexes O-H CO where the C atom is preferentially attached to the proton. Therefore, the heteronuclear magnetic dipole interaction between the proton and the 13C nucleus of the ~3CO molecule has to be taken into account besides the chemical shift.anisotropy. The spectrum numerically calculated for this complex with a H-C hydrogen bond distance rH_c of 0.21 ___ 0.01 nm and AOc ~ 370 ppm excellently agrees [24] with the experimentally observed spectrum. This H-C hydrogen bond distance is in complete accordance with the predictions of quantum chemical calculations [25-27]. Furthermore, it is remarkable that AOc increases compared with physisorbed ~3CO. It can be stated that variable-temperature 13C NMR spectroscopy allows the study of the geometry and the thermal motions of the adsorption complexes formed by CO molecules hydrogen bonded to surface hydroxyl groups.
3.3. The influence of C2Cl 4 on the IH MAS NMR spectra of zeolites Fig. 2 shows the 1H MAS NMR spectrum of zeolite 0.3 HNa-Y loaded with 8 molecules C2CI4 per unit cell which is less than the actual concentration of ca. 17 bridging hydroxyl groups per unit cell. Obviously, a part of the signal at ~H = 3.9 ppm due to bridging hydroxyl groups in the large cavities is shifted to a position of ~H c2c~4 = 5.5 ppm.
Figure 2. 1H MAS NMR spectrum of zeolite 0.3 HNa-Y loaded with 8 molecules C2C14 per unit cell measured at 123 K.
. . . .
i
8
. . . .
i
7
. . . .
i
6
. . . . .
i
. . . .
5
i
. . . .
4
/ ppm
|
3
. . . .
i , , , , , i
2
. . . .
1
17 The spectrum measured at room temperature exhibits only one line at 4.5 ppm instead of the two signals at 3.9 and 5.5 ppm which shows that the C2C14molecules exchange rapidly between the bridging hydroxyl groups at 293 K. In contrast, the presence of the two well resolved signals at 123 K evidences that the exchange processes of the C2C14 molecules between the bridging hydroxyl groups are slow. Furthermore, it could be shown that the induced chemical shift becomes independent of the temperature for T < 150 K, i.e., it can be assumed that the maximum value of A8 is reached. Fig. 3 demonstrates that the correlation between A8 and (-Av) is given by a straight line with a slope of B = 0.01 [28] as it was predicted above (cf. eq. (6)). Therefore, the induced chemical shift A6 measured at 123 K for samples loaded with C2C14 is not only a qualitative measure for the strength of acidity of free surface hydroxyl groups. It can also be used for the calculation of the deprotonation energy according to eq. (5) since Av and n VSiOHcan be replaced by A~ and A~SiOH , respectively. An induced chemical shift of AbsioH = 0.75 ppm was determined for SiOH groups [28]. The induced chemical shift A 6 amounts to 1.6 ppm for bridging hydroxyl groups in the large cavities of 0.3 HNa-Y. From eq. (5) it follows that AEDp ~ 1250 kJ mo1-1 which is close to the value of ca. 1240 kJ mol -~ obtained with bH = 3.9 ppm by using eq. (4). Furthermore, it can be suggested to make use of 8H C2C14as a sensitive qualitative measure for the strength of acidity since both 8H and n 8 reflect the strength of acidity of free surface hydroxyl groups.
2,2
-
2,0
9
1,8
9
9
1,6
E Q. 1,4 ,,o 1,2 1,0 0,8 0,6 n
60
80
100
120
140
-Av / cm
160
180
200
220
-1
Figure 3. Correlation between the induced 1H NMR chemical shift A8 and the induced wavenumber shift nv caused by adsorbed C2C14 for free surface hydroxyl groups in zeolites.
18 ACKNOWLEDGEMENT The author wishes to express his gratitude to Prof. Dr. Dr. H. Pfeifer and Dr. B. Staudte for helpful discussions and to Mr M. Koch and Ms H. Sachsenr6der for excellent experimental assistance. Financial support by "Deutsche Forschungsgemeinschaft" (SFB 294 "MolekiJle in Wechselwirkung mit Grenzflfichen") is highly appreciated. REFERENCES .
2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21. 22. 23.
24. 25. 26. 27. 28.
H. Pfeifer, NMR Basic Principles and Progress, Vol. 31, Springer, Berlin 1994., p.31. H.G. Karge, Stud. Surf. Sci. Catal., 65 (1991) 133. J. Sauer, J. Mol. Catal., 54 (1989) 312. V.B. Kazansky, Kinetika i Kataliz, 21 (1980) 159. V.B. Kazansky, Stud. Surf. Sci. Catal., 85 (1994) 251. P.A. Jacobs, Catal. Rev.-Sci. Eng., 24 (1982) 415. P.A. Jacobs and W.J. Mortier, Zeolites, 2 (1982) 226. H. Pfeifer, D. Freude and M. Hunger, Zeolites, 5 (1985) 274. D. Freude, M. Hunger and H. Pfeifer, Z. Phys. Chemie NF, 152 (1987) 171. U. Fleischer, W. Kutzelnigg, A. Bleiber and J. Sauer, J. Am. Chem. Soc., 115 (1993) 7833. J. Sauer and J.-R. Hill, Chem. Phys. Lett., 218 (1994) 333. E.A. Paukshtis and E.N. Yurchenko, Usp. Khim., 52 (1983) 426. E. Brunner and H. Pfeifer, Z. Phys. Chemie, in press. E.A. Paukshtis and E.N. Yurchenko, React. Kinet. Catal. Lett., 16 (1981) 131. L. KubelkovS., S. Beran and J.A. Lercher, Zeolites, 9 (1989) 539. M.A. Makarova, A. Garforth, V.L. Zholobenko, J. Dwyer, G.J. Earl and D. Rawlence, Stud. Surf. Sci. Catal., 84 (1994) 365. E. Brunner, H.G. Karge and H. Pfeifer, Z. Phys. Chemie, 176 (1992) 173. J.L. White, L.W. Beck and J.F. Haw, J. Am. Chem. Soc., 114 (1992) 6182. L.M. Kustov, V.B. Kazansky, S. Beran, L. Kubelkovfi and P. Jir~, J. Phys. Chem., 91 (1987) 5247. I. Mirsojew, S. Ernst, J. Weitkamp and H. Kn6zinger, Catal. Lett., 24 (1994) 235. E. Brunner, J. Mol. Struct., in press. M. Koch, E. Brunner, D. Fenzke, H. Pfeifer and B. Staudte, Stud. Surf. Sci. Catal., 84 (1994) 709. A.J. Beeler, A.M. Orendt, D.M. Grant, P.W. Cutts, J. Michl, K.W. Zilm, J.W. Downing, J.C. Facelli, M.S. Schindler and W. Kutzelnigg, J. Am. Chem. Soc., 106 (1984) 7672. M. Koch, E. Brunner, H. Pfeifer and D. Zscherpel, Chem. Phys. Lett., 228 (1994) 501. S. Bates and J. Dwyer, J. Phys. Chem., 97 (1993) 5897. P. Geerlings, N. Tariel, A. Botrel, R. Lissillour and W.J. Mortier, J. Phys. Chem., 88 (1984) 5752. K.M. Neyman, P. Strodel, S.P. Ruzankin, N. Schlensog, H. Kn6zinger and N. ROsch, Catal. Lett., 31 (1995) 273. H. Sachsenr6der, E. Brunner, H. Pfeifer and B. Staudte, in preparation.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
19
D e t e r m i n a t i o n o f the e n v i r o n m e n t o f titanium a t o m s in TS-1 silicalite by Ti Kedge X - r a y A b s o r p t i o n S p e c t r o s c o p y , 29Si and 1H N u c l e a r M a g n e t i c R e s o n a n c e . L. Le Noc a, C. Cartier dit Moulin a'b, S. Solomykina a, D. Trong On a, C. Lortie a, S. Lessard a and L. Bonneviot a aFacult6 des Sciences et G6nie, Universit6 Laval, G 1K 7P4 Sainte Foy (Qc), Canada bLaboratoire pour l'Utilisation du Rayonnement Electromagn6tique, CNRS-CEA-MENJS, B~timent 209d, 91405 Orsay Cedex, France The titanium environment and the modification engendered by the framework when this element is incorporated in a silicalite of orthorombic MFI structure were investigated using Ti K-edge X-ray Absorption, 298i and IH MAS NMR spectroscopy. A multiple scattering analysis of the EXAFS signal reveals that the titanium occupies a substitutional site characterized by Ti-O-Si bond angle, Ti-O and O-Si average distances consistent with a lattice expansion. The defects concentration remains constant and independent of the Ti loading. The proton NMR spectra of S-1 is characterized by narrow resonance lines whose relative intensities are modified in TS-I which indicate either the presence of new TiOH groups and/or a redistribution of the internal SiOH groups.
INTRODUCTION Microporous titanium silicalites of MFI or MEL structures, TS-1 and TS-2 respectively, have attracted many scientists owing to their unique capability to catalyze the oxyfunctionalization reactions of alkanes using H202 as oxidant. Despite the number of new titanium silicalites with larger and larger pore sizes such as Ti-beta, titanium mesoporous materials such as Ti-MCM-41, Ti-MCM-48 or high surface area amorphous TiO2-SiO2, no other materials were active for this demanding reaction [1-4]. The presence of micropores might be necessary for oxyfunctionalization to take place, though a specific local environment around titanium might as well be required for these reactions. These materials exhibit an IR band at 960 cm 1. It is assigned to a local vibration mode of the asymmetric stretching of a SiO4 unit linked to either a Ti 4+, a V 4+ or a Cr 3+ ion in amorphous or crystallyzed systems [57]. Consequently, this band is not an intrisic characteristic of titanium silicalite materials. The Ti isomorphous substitution for Si in these systems is a widely shared belief based on a conjunction of facts obtained from a panel of techniques such as XRD [8], IR, UV-visible, XPS [9], EXAFS [10], XANES [10] rather than on a direct proof. Recently, using the multiple scattering (MS) theory to analyze the second shell of neighbours around the titanium
20
in a TS-1, some of us calculated an average Ti-O-Si angle of about 160 ~ consistent with the isomorphous substitution proposal [~1]. Refined MS calculations on TS-1 free of Ti extraframework species, 29Si and H MAS NMR investigations of the framework modifications in presence of Ti are reported here. EXPERIMENTALS Three titanium silicalites with a Ti/(Ti+Si) atom ratio of 0.005, 0.010 and 0.015 were synthesized from a gel containing a mixture of TEOS, TEOT and TPAOH in propanol. Water was added. The hydrothermal crystallization was performed in a Teflon-lined stainless steel autoclave at 175~ for 4 days. The solid was filtered, washed and calcined at 5Q0~ The XRD recorded on a Rigaku D-Max IIIVC X-ray spectrometer revealed a crystallinity of about 95%. These samples exhibit features that characterizes TS-1 materials without extraframework Ti species, i) an MFI orthorhombic structure with a unit cell expansion of 25 A 3 per Ti, ii) an IR band at 960 cm -t and iii) no UV bands in the 270-400 nm UV range where the electronic transition of TiO2 anatase arises and iv) the characteristic X-ray near edge features of tetrahedral environment [ 10]. The X-ray Absorption measurements at the Ti K-edge were performed at the radiation synchrotron facility of the LURE (France). The white radiation was monochromatized using a Si(111) two crystals monochromator and harmonic rejection was obtained by detuning the crystals. The EXAFS signals were measured in transmission mode from 4800 to 5800 eV with 2 eV steps on samples pressed into pellets. The samples were dehydrated under vacuum at 500~ and transferred to a leak tight XAS cell under controlled atmosphere. The signal was extracted and normalized using a software package developed by Michalowicz [12]. The Fourier transforms were calculated after applying a parametrized Kaiser window function (t 3.7) between 3.16 and 14.20 A -1. The first shell was analyzed using the single scattering (SS) theory combined to an automated mean square minimization curve fitting process [12]. The second shell analysis that necessitated MS calculations were performed using the FEFF6 code from Rehr et al [ 13]. These calculations are usually performed on a priori known structures. Therefore the structures were generated using Cerius 2 TM, a molecular modeling package from Molecular Simulations. A trial and error approach was adopted to reach the structure that led to the best fit of the experimental data. The NMR measurements were also performed on TS-1 dehydrated at 500~ and transferred under controlled atmosphere into the rotors. No rehydration occured during the experiments as it was probed by tH NMR. The MAS NMR spectra were obtained at room temperature using a Bruker ASX 300. The rotors were spun at a rotation frequency of 4kHz. For 298i NMR, an onepulse sequence with a n/2 pulse of 5ps was used. The cycle time of 60s allows a full relaxation of the spins of all the silicon species. IH spectra were recorded following an echo sequence (n/2-x-n) where the echo time x is equal to the inverse of the spin rate, n/2 is 51as and the cycle time is fixed to 2.5s (full relaxation). The shifts are referenced to an external TMS standard.
21
~
:, , i , , . , i , , ~, i , ,', _ i r , , I , ,
9X - 0 . 4
_
:.i-
1.2
..'" ,,
,
i
4
'..
',..."r
i,
'..
....,- ......
,
6
I t i
8
,
12 I. ' ' . ' '
",..,. ....... 9.........
i
l,
10
,
I
~"
I '' ' ' I ....
~, ,.r,___
_
.
, , ...... i'1
12
....
~
14
0
.e
i
I
2
o
I . . . .
4
3
-
5
R(A)
k(A -i)
Figure 2. Module of forward transforms (uncorrected for phase the experimental (solid line) and FEFF6 (dots) model shown in fig.
Figure 1. Normalized EXAFS spectra of [1.5] TS-1 (solid line) compared to SS and MS-FEFF6 calculations using a [Ti(OSi)4] cluster with a geometry given in the text.
.4 pl i
Fourier shift) of the MS1.
........ , ....... .... ;
I II I I I'I I I'I I I I'"I I I'I I I I'I I l,lal i
f..t.,
"g o 2
4 1
2.s
3
RCA)
3.s
1
ltliltltlilll tt lit ill= ---Ii -
I
4
2.5
3
R C A ) 3.s
4
Figure 3. Imaginary part of forward Fourier transforms of the second shell of experimental (solid line) and MS-FEFF6 calculations (dots) for sets of Si-O distance and Ti-O-Si angle, a) 1.638 A and 161 ~ (as in fig. 1 and 2) and b) 1.62 A and 163 ~ respectively.
RESULTS
The X-ray near edge region for the three dehydrated TS-1 not shown here are identical and similar to those shown in the litterature for extraframework Ti free TS [10]. In addition, the similarity of the XANES of TS-1 and a model compound, the hexadecaphenyloctasiloxyspiro(9,9)titanium(IV) (HDPOSST), made of a tetrahedral [Ti(OSi)4] core strongly suggests that the titanium in the silicalite framework adopts the same symmetry and coordination compatible with a substitutional site [11]. The SS analysis of the first shell EXAFS
22
contribution led to a Ti-O distance of 1.80 +0.01 /~ also consistent with a tetrahedral environment. The multiple scattering calculation was proved to be necessary to reproduce the EXAFS signal of the HDPOSST [11]. This was attributed to widely open Ti-O-Si angles spanning in the 156-173 ~ range. A satisfying fit was obtained for calculations restricted to the tetrahedral [Ti(OSi)4 ] core of this molecule (Rmax = 4/~). A similar quality of fit was also obtained using average values 1.782/~ for Ti-O distance and 166 ~ for Ti-O-Si angle instead of the actual values. This demonstrated that the technique provides average values. A [Ti(OSi)4] cluster of atoms was also used to simulate the experimental EXAFS data of TS-1 samples (Fig. 1 and 2). To improve the match with the experimental data, the Ti-O distance and the Ti-O-Si angle were optimized resulting in a new set of 1.805 A and 163 ~ Further refinements were obtained by trial and error changing the O-Si distance as well. This led to a new O-Si distance of 1.638 ,~ and a Ti-O-Si angle of 161 ~ The accuracy of the process was estimated to be + 0.01 A on the distance and • 1~ on the angle. The Debye-Waller factors (DWF) that rely on the thermal agitation and structural disorder were found to be ol 2 = 0.00155 for the first shell and ~22 = 0.0045 for the second shell (S02 = 0.85) for the model compound [11]. For the TS-1 samples the DWF of the second shell had to be increased up to 0.0089. Keeping ol 2 and or22 the same as for the model compound would have led to 3 Si, assuming a [Ti(OSi)3(OH)] type of site. The 29Si MAS NMR was performed to identify the structural defects from vacancies of silicon implying nested OH or broken Si-O-Si bridges. The 29Si NMR spectra (fig.4) of the titanium free silicalite (S-l) and the TS-1 materials exhibit an intense and broad signal at -113 ppm assigned to Q4 [Si(OSi)4] species and a less intense signal at -103 ppm assigned to Q3 [Si(OSi)3OH ] species. No geminal silanol species were observed in the TS-1 or S-1 samples, even when cross polarization was used. The number of Q3 species is hardly constant and nearly equal to 8 per unit cell (8.2, 7.9, 7.2, 7.8 +1 for S-I, [0.5] TS-1, [1.0] TS-1 and [1.5] TS-1 respectively). Assuming a number of at least 3 Ti-O-Si bridges per Ti, the [Si(OSi)3(OTi)] species would already increase the Q3 signal by about 50% if they were to resonate at the same frequency. Consequently, the [Si(OSi)3(OTi)] species contribute to the Q4 signal intensity. The mformatlon taken from the Q signal is therefore exclusively related to the number of silanol species found at a nearly constant concentration whatever the titanium loading. The zeolites have been dehydrated during 12 hours at 500~ in vacuum. An analysis by mass spectrometry of the desorption under a flow of pure helium gas between 25 and 500~ (heating rate of 4~ demonstrates that all the physisorbed water is evacuated at 100~ and the water from the condensation of neighbouring silanols is eliminated after two hours at 500~ It can be pointed out that some trace of organic template is also observed and disappears at 400~ The structural defects observed by IH NMR correspond to terminal SiOH and possibly TiOH hydroxyls which are isolated or difficult to eliminate for structural reasons (lattice constraints, bad conformation of neighbouring hydroxyl groups,...). For the pure silicalite S-l, three components can be seen at 1.8 ppm (a), 2.2 ppm (b), and around 3.2 ppm (c) with the ratio 1/3 for each line (fig.5). A strong steaming (175~ in an autoclave in presence of water: conditions of crystallization) was performed leading to the monoclinic MFI structure. This has been confirmed by 29Si MAS NMR: 17 peaks or 9
9
3
9
23 10 TS11.5%
1.0
~TS10.5%
8
Q4 $1
0.8 A [, . ! . . . . [ ~ 5 t~ 0.6 ~ - 9 0 -100
56 .
4
3
2
,
,
-11
i""
r
y_=
L
e-
4
0.4
2
0.2 -
,,,,
0.0 0
!
5
4
3
2
1
chemical shift (ppm/TMS)
Figure 4. IH MAS-NMR spectra of the silicalites S-l, [0.5] TS-1 and [1.5] TS-I" spectra normalized on the weight of sample.
-80
-90
,
I
I
I
-100
-110
-120
-130
chemical shift (ppm/TMS)
Figure 5. 29Si MAS-NMR spectra of the silicalites S- 1 and [1.5] TS- 1.
shoulders with a total intensity of 24 are clearly visible instead of the Q4 broad line. The Q3 signal is absent. The receiver gain used for the IH NMR is 32 times greater than for the silicalite with 8% of defects. Surprisingly, these experiments show that the terminal silanols can resonate within a large window (1.5-4.5 ppm), far from the common value of 2 ppm. After one year of air exposure, the monoclinic silicalite progressively evolves toward the orthorhombic structure, containing 6% of Q3. The corresponding 'H NMR spectra exhibit the same components as the original silicalite with a higher proportion of the species giving rise to line c. It is unprobable that vacancies of silicon could have been created at room temperature in this structure, so the line c can not be assigned to strongly interacting nested OH around vacancies. Furthermore, it is worthwhile to notice that contamination by water lead to a well defined signal at 3.5 ppm, broader than those observed for the monoclinic silicalite and narrower than the line c for the orthorhombic silicalite. Finally, all the defects a, b and c seem to be natural defects of the structure. They probably correspond to terminal silanols in different conformations, arising from non-intact Si-O-Si bridges. The line a corresponds to defects which are easier to eliminate than the defects of type b and c. An ambiguity resides the high chemical shift of the line c (which could be due to strong interacting silanols), the difficulty to eliminate these defects and the fact that they do not seem to originate from silanol vacancies. The lH NMR spectra of the titanium containing silicalites show the same components as the pure silicalite. In this case, the proton can be a silanol proton or a titanol proton. The anatase TiO2 is characterized by two lines, one at 6.4 ppm from Ti-OH-Ti bridges and another
24 one from terminal TiOH groups at 2.3 ppm [16-17]. For anatase free TS-1, we only expect terminal TiOH species in the region of 2 ppm, their effective chemical shift depending on the structural environment as it is the case for the silanol protons. There is indeed no evidence of a signal from anatase clusters at about 6 ppm. A continuous increase of line a intensity with an increasing titanium content in the silicalite is observed (fig.5). Conversely and to a lesser extent, it seems that the line b decreases, while no significant change occurs for line c. The precision on the Q3 defects number does not allow to correlate the proton and Q3 signal intensities with the titanium loading. Moreover, these defects may be differently distributed among the type a, b and c, possibly explaining that the increase of line a intensity is not proportionnal to the Ti loading. Anyhow, the NMR data can be interpreted both ways as the result of formation of titanol species, or increase of type a silanol defects. It seems that no specific structural defects are produced in presence of titanium. DISCUSSION Within the range of 0.005-0.015 Ti/(Si+Ti) ratios, the TS-I investigated here exhibit the expected XRD, IR and UV-visible characteristics of TS-1 materials free of extraframework species. Their XANES spectra similar to the XANES spectrum of the model compound HDPOSST confirm this statement and bring further supports for the Ti isomorphous site occupancy [11]. The average Ti-O-Si angle decreases from 166 ~ in the molecular HDPOSST compound to 161 ~ in the TS-1, getting close to the average Si-O-Si angle of 154 ~ in the titanium free silicalite. This reveals the existence of a local pressure exerted on the Ti site by the lattice. The average Ti-Si distance of 3.38 A is however longer than the average Si-Si distance of 3.10 A and correspond to a local expansion of 37/~3 per Ti. The lattice is obviously relaxed since an actual 25 A 3 lattice expansion is measured. The 29Si NMR already reveals that the S-I framework relaxes from monoclinic to orthorhombic by SiO-Si bond breaking and narrowing of the Si-O-Si bond angle distribution. No further relaxation seems to occur when Ti is incorporated in the lattice according to the constant Q3 concentration. This situation could be explained by a local relaxation on the Ti site implying only a small rearrangement of the lattice. From this model, a [Ti(OSi)3(OH)] local (open) model is more probable because of the broken Ti-O-Si bond than the [Ti(OSi)4] (closed) model. In addition, according to the synthesis route that randomly distribute the titanium in the gel before cristallization, it is more likely that there is no site discrimination for the substitution. Unfortunately, since the coordination number and the DWF are correlated, it is impossible to differentiate between the closed and the open Ti site models from EXAFS. Moreover, the proton NMR does not bring any definitive proof of the existence of TiOH since a new SiOH distribution might as well explain the increase of line a in the spectra (fig.5).
25 CONCLUSION The MS calculations at the Ti K-edge EXAFS and the MAS NMR investigations at the IH nuclei lead to the conclusion that the titanium ions are located in framework substitutional sites of the TS-1 materials. It is more likely that Ti is randomly located in the structure. However, it seems that the relaxation of the lattice might occur by T-O-T bridge breaking preferably involving more Ti sites that are obviously more constrained than silicon sites with a roughly constant lattice defect concentration.
29Si and
1. 2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17.
T. Blasco, M.A. Camblor, A. Corma and J. P6rez-Pariente. J. Am. Chem. Soc. 115 (1993) 11806. P.T. Tanev, M. Chibwe and T.J. Pinnavaia, Nature 368 (1994) 321. J.S. Reddy, A. Dicko and/~. Sayari, Prepr., Am. Chem. Soc., Div. Petrol. Chem. 40 (1995) 225. R. Hutter, D.C. Dutoit, T. Mallat, M. Schneider and A. Baiker, J. Chem. Soc., Chem. Commun. (1995) 163. M.R. Boccuti, K.M. Rao, A. Zecchina, G. Leofanti and G. Petrini, Stud. Surf. Sci. Catal. 48 (1989) 133. P.R. Hari Prasad Rao and A.V. Ramaswamy, J. Chem. Sot., Chem Commun. (1992) 1245. Y. Chapu, A. Tuel, Y. Ben Taarit and C. Naccache, Zeolites 14 (1994) 349. R. Millini, E. Massara Previde, G. Perego and G. Bellussi, J. Catal. 84 (1994) 501. D. Trong On, L. Bonneviot, A. Bittar, A. Sayari and S. Kaliaguine, J. Mol. Catal. 74 (1992) 223. S. Bordiga, S. Coluccia, C. Lamberti, L. Marchese, A. Zecchina, F. Buffa, F. Genoni, G. Leofanti, G. Petrini, G. Vlaic, J. Phys. Chem. 98 (1994) 4125. C. Cartier, C. Lortie, D. Trong On, H. Dexpert and L. Bonneviot, Physica B 208-209 (1995) 653. A. Michalowicz, Logiciels pour la chimie: EXAFS pour le Mac, Soci6t6 frangaise de chimie (1991) 116. P.A. O'Day, J.J. Rehr, S.I. Zabinsky and G.E. Brown Jr., J. Am. Chem. Soc. 116 (1994) 2938. G.E. Maciel, D.W. Sindorf, J. Am. Chem. Sot., 102 (1980) 7606. G. Engelhardt, D. Michel, High-Resolution Solid-State NMR of Silicates and Zeolites, Wiley Interscience, New York (1987). V.M. Mastikhin, A.V. Nosov, React. Kinet. Lett., 46 (1992) 123. S. Haukka, E.L. Lakomaa, A. Root, J. Phys. Chem., 97 (1993) 5085.
This page intentionally left blank
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
A n in situ
13C l~lmS N M R
27
study of toluene alkylation with m e t h a n o l over H -
ZSM-11 Irina I. Ivanova # and Avelino Corma Instituto de Technologia Quimica, UPV-CSIC, Avd. los Naranjos s/n, 46022 Valencia, Spain
13C MAS NMR has been performed in situ to investigate the reaction of toluene with methanol (MeOH)over H-ZSM-11 catalyst. The identification of the main reaction products and intermediates and the quantification of the NMR results provide new information concerning the nature of the methylating agents, the primary products of alkylation and the whole reaction network. During the initial stages of the reaction, methanol partially converts to dimethyl ether (DME).The reaction then proceeds via two parallel reaction pathways. The first pathway which is the major one includes toluene methylation with DME or MeOH to yield o- and p-xylenes in the statistical ratio of two to one. The primarily formed xylenes undergo isomerization and further alkylation to tri- and tetramethylbenzenes. The observation of diphenylmethane-like species as reaction intermediates suggests transalkylation of alkylaromatics. The second reaction pathway includes toluene alkylation with the fragments formed upon methanol conversion to hydrocarbons and thus leads to various alkyltoluenes. The latter, in turn, undergo dealkylation, fragmentation and transalkylation to yield mainly xylenes, ethyltoluenes and polymethylbenzenes.
1. INTRODUCTION Toluene alkylation with methanol over pentasil type catalysts has been thoroughly studied during the last decade [1-12]. Attention was focused mainly on the application of these catalysts in the selective production of p-xylene [1-7]. Mechanistic studies have been limited because the reaction pattern is affected significantly by diffusion [4], and the products observed at the outlet of convensional continuous flow reactors, do not reflect the real kinetic situation on the catalyst. Information on this situation can now be obtained by means of recently developed in situ spectroscopic techniques [8-12]. This study aims to clarify the mechanism of toluene alkylation with methanol using in situ 13C M.AS NMR technique. The attention is focused on the following main aspects: 1) identification of the reaction pathways operating under the NMR/batch conditions; 2) identification of the reaction intermediates which may play the role of alkylating agents; 3) identification of the primary and secondary reaction products.
# On leave from Moscow State University,Russia
28 2. EXPERIMENTAL 2.1. Materials The study was performed on H-ZSM-11 catalyst with Si/AI ratio equal to 23. The catalyst was characterized using XRD, electron microscopy, FTIR, solid state 27A1 and 29Si MAS NMR, sorption of n-hexane and NH3 TPD. Methanol 13C (99.9% - enriched) used as labelled reactant was obtained form ICON Services Iiac. Natural abundance 13C toluene and dimethyl ether were obtained from Aldrich Chemical Company and Linde Technische gase, respectively.
2.2. Controlled-atmosphere 13CMAS NMR measurements Controlled atmosphere NMR experiments were performed in sealed glass NMR cells containing a catalyst and an adsorbate, and fitting precisely into MAS rotors. In a typical experiment, the powdered catalyst was packed into the NMR tube (Wilmad, with constriction), and evacuated to a final pressure of 10 -5 Tort after heating for 10 h at 573 K. Thereafter, the catalyst was cooled down to 298 K and the reactants were subsequently adsorbed. Toluene and methanol were dosed gravimetrically, whereas dimethyl ether was dosed volumetrically. Quantitative adsorption was ensured by cooling the sample to 77 K. After loading the reactants, the NMR cells maintained at 77 K to avoid local overheating were carefully sealed to achieve proper balance and high spinning rates in the MAS NMR probe. 13C MAS NMR measurements were carried out on a Varian VXR-400S WB spectrometer operating at 100.6 MHz. Spinning rates were within 4.5 - 5 kHz. Quantitative conditions were achieved using high-power gated proton-decoupling with suppressed NOE effect (3 ~ts 90 ~ pulse, recycling delay 6 s). Some non-lH-decoupled spectra were recorded and the observed multiplet patterns were analyzed to identify reaction products and intermediates. The assignments of some signals were confirmed by the direct adsorption of model compounds on the same catalyst in a separate set of experiments (e.g. in case of xylene isomers). Variable-temperature (298 - 387 K) and cross-polarization (contact time 5 ms) experiments were performed to distinguish between the species with different mobilities. The reaction was carried out by heating the sealed NMR cells outside of the spectrometer in the temperature range of 373 - 673 K. The 13C MAS NMR measurements were performed at lower temperatures (298 or 387 K) after quenching of the sample cells. After collection of the NMR data, the NMR cells were returned to reaction conditions. Two different reaction protocols were used. In the first one, the temperature was increased in a stepwise manner from 298 to 673 K, the NMR spectra being recorded after heating for 10 min at each temperature step. In the other experiments, the sample was rapidly heated to a final temperature (433 K) and maintained at this temperature for various periods of time (2 - 1400 min). 13C NMR spectra were recorded over the time course of the reaction. The first experimental mode showed more clearly a sequence of products, while the second one facilitated a comparison of reaction kinetics. The list of experiments is reported in Table 1. Quantification of the NMR results requires a number of definitions which are listed below: Conversion of methanol 13C at time t (Xt)was determined as, Xt = (1 - Im,t/Im,0)'100 [%], where Im,t corresponds to the integral intensity of the NMR line assigned to methanol in the NMR spectrum observed after heating for t min, Ir,0 corresponds to the integral intensity of methanol resonance in the initial spectrum. Yield of reaction product p at time t (Yp,t) was determined as methanol 13C conversion into this product,
29
Yp,t = (Ip,t/Im,0)" 100 [%], where Ip,t corresponds to the integral intensity of the product p resonance in the NMR spectrum observed after heating for t min. Table 1 List of experiments Experi- Catalyst
Reactants (molec./u.c.) Toluene MeOH13C
Reaction protocol
DME
Tspectra
ment
(g)
registr. (K)
A
0.02
20
13
-
stepwise temp. rise: 298-673 K
298
B
0.03
14
-
7
stepwise temp. rise 298-483 K
298
C
0.03
17
9
-
progressive increase of reaction
298
D
0.02
17
9
-
progressive increase of reaction
time; Treact.=433 K 387
time; Treact.=433 K
3. RESULTS AND DISCUSSION 3.1. Identification of the reaction products and intermediates. Reaction network 13CMAS NMR spectrum observed after adsorption of reactants over H - Z S M - 1 1 at 293 K (Fig. 1, Sample A) shows 5 narrow resonance lines at ca. 21, 125.5, 128.4, 129.2 and 137.8 ppm corresponding to unlabelled toluene and a broad signal at ca. 51 ppm corresponding to methanol 13C [13]. After heating the NMR cell to 373 K, methanol starts to convert to DME, evidenced by the appearance of the broad NMR line at ca. 60.3 ppm, as was also observed for H - Z S M - 5 zeolites when methanol was the only reactant [14, 15]. The line corresponding to DME reaches its maximum intensity at 413 K and then remains unchanged until alkylation begins. Alkylation starts at 433 K. The primary products are o-xylene and p-xylene confirmed by the resonance lines at 19.3 and 20.7 ppm, respectively. In the aromatic part of the spectra, formation of o-xylene is evidenced by the appearance of weak resonances at 126 and 129.8 ppm; The lines corresponding to p-xylene overlap with toluene resonances. Interesting, that observation of the primary products depends on the reaction protocol used (Table 1). This is discussed further in w 3.3. Further heating to 483 K results in the observation of new resonances at ca. 41.3, 30, 24 and 14 ppm. The latter three lines are related to conversion of methanol or DME to hydrocarbons [14, 15]. The narrow resonance at 24 ppm is assigned to i-butane, the major product of methanol conversion. The broad lines at ca. 30 and 14 ppm correspond to very rigid species as confirmed by experiments with cross-polarization, and may be attributed to overlapping species stemming from various longer chain hydrocarbons. The NMR line at 41.3 ppm can not be associated with the products of methanol conversion and is more likely due to diphenylmethane-like species [13] formed from toluene and/or xylenes. After heating to 523 K methanol consumption is terminated. The lines corresponding to long chain hydrocarbons disappear, indicating their cracking. As a result, weak resonances corresponding to alkyltoluenes are observed, pointing on toluene alkylation with the fragments formed upon cracking [16]. The most intensive resonances are attributed to sec-
30 butyltoluenes (42.1, 31.6, 22.2, 12.3 ppm), n-propyltoluenes (38.3, 24.6, 14 ppm), isopropyltoluenes (34.3, 24.6 ppm) and ethyltoluenes (29, 16 ppm) [13]. Formation of alkyltoluenes is accompanied by growing of the resonances corresponding to i-butane (24 ppm) and propane (16-17 ppm).
Sample A
~.
,~
673
K
523
K. . . . . . . . .
433
K
/
21.2
" " '-
"-
" -'- -- , 4
\
S
___-/AX..__./x~
. . . . . . . . . . .
. . . . .
,,
373 .
'
140
'
"
"
l
130
'
'
"
"
I
120
.
.
S I '
,, , ,
.
K .
.
]9
~
.....
....
/ ~\
_0_' .
I
"
'
'
'
I
60
'
'
'
"
I
"
'
'
'
I
40
'
'
'
'
1
'
'
'
'
I
20
'
'
'
"
9
ppm
Figure 1. 13C MAS NMR spectra observed before and after reaction of methanol 13C and toluene over H-ZSM-11 at progressively increasing temperatures. *- denotes spinning sidebands. Isomerization of xylenes begins in the temperature range of 523 - 573 K as evidenced by the appearance of the growing NMR lines at ca. 21.2, 126.4 and 130 ppm, corresponding to m-xylene [13]. At this reaction step, the lines corresponding to trimethylbenzenes and tetramethylbenzenes mainly 1,2,4-trimethylbenzene, and 1,2,4,5-tetramethylbenzene (growing shoulder at ca. 19 ppm [13]) also begin to appear. Further heating to 623 and 673 K leads to an equilibrium mixture of xylenes (p:o:m=23.7:52.8:23.5), formation of more polymethylbenzenes, and to fragmentation and dealkylation of butyl- and propyltoluenes to give methyl- and ethylsubstituted aromatics. Meanwhile the line corresponding to diphenylmethane disappears. The reaction network presented in Figure 2 rationalizes our experimental observations. At the initial stages of the reaction, methanol readily condenses to give DME and water. Both
31
methanol and DME may be responsible for further reaction proceeding via two parallel pathways: 1) toluene methylation and 2) conversion to hydrocarbons. The first reaction pathway leads to o- and p-xylenes as the primary products. At higher temperatures, o- and p-xylene isomerize to m-xylene, to give an equilibrium mixture of xylenes. The timing of the appearance and disappearance of small amounts of diphenylmethane like species is indicative of their intermediary role in isomerization. This gives further evidence that some xylene formation on zeolites may occur via a bimolecular transalkylation mechanism [17-19]. Xylenes in their turn undergo further alkylation or transalkylation to yield tri- and tetramethylbenzenes.
J
/
IT~ 1~73~K MeOHI ~--"" ( DME (o-,p-XylenesI "',~ .~ 473K...~ t_ ~-..... 523-673K IHydrocarbons ) I Diphenylmethanes)-~~ ~ 523-673K 1 I Tri-andtelramethylbenzenes 1 IEthyl-rpropyl-andbutyltoluenes '~ 673K .~ I Xylenes(eq.mixt.),ethyltoluenesandpoly'nelhylbenzenes I Figure 2. Reaction network.
The second route leads to small amounts of i-butane and some longer chain hydrocarbons, which upon cracking may yield lower alkanes and carbenium ion like species. Toluene acts as a trap for these species, as was observed for benzene in the course of the cracking of propylene oligomers [16]. As a result, butyl-, propyl-, and ethyltoluenes are formed. At higher temperatures, alkyltoluenes undergo dealkylation, fragmentation and transalkylation to yield mainly xylenes, ethyltoluenes and polymethylbenzenes. The final products observed at high temperatures (673 K) in our NMRfoatch experiment correspond to those observed in continuous-flow reactor tests [3], suggesting that the reaction proceeds in a similar way under both experimental conditions. The advantage of the in situ NMR techniques is the possibility to tailor specifically the reaction protocol which enables one to minimize superimposing of the parallel and consecutive reaction steps. As a result, the individual steps of the reaction can be followed in separate experiments and the reaction intermediates can be identified. The optimal conditions for the investigation of the individual reaction steps were determined to be 433-453 K for alkylation, 473-523 K for methanol conversion to hydrocarbons, 523-573 K for isomerization and hydrocabons cracking, and above 573 K for transalkylation dealkylation and fragmentation. The alkylation step will be considered in more detail.
32
3.2. A l k y l a t i n g agents
It is currently accepted that toluene ring-alkylation with methanol proceed via chemisorption of methanol on the acid sites, followed by formation of surface active species such as methoxy groups [21-23] or methoxonium ions [10, 11, 20], which can further react with weakly adsorbed toluene. On the other hand, it is known that DME is always present in abundance on the onset of xylenes formation [9, 10, 21] and there are indications that observation of DME can be associated with ring alkylation [8, 24]. Our results (Figs. 1,2) are also in favour of DME intermediary role in alkylation. Two other experiments were performed to check this hypothesis. In the first one, DME was adsorbed together with toluene over H - Z S M - 1 1 catalyst and the reaction was carried out as in experiment A (Table 1, Sample B). The aliphatic regions of the 13C MAS NMR spectra are presented in Fig. 3. The initial spectrum obtained after adsorption of reactants shows a broad NMR line at ca. 60.3 ppm and narrow line at ca. 21 ppm, assigned previously to DME and methyl group of toluene, respectively. Heating to 453 K results in a partial conversion of DME to p - and o-xylenes confirmed by the resonances at 20.7 and 19.3 ppm, respectively. No resonance line corresponding to MeOH is detected, possibly because the latter is rapidly converted back to DME at 453 K, as was observed in experiment A. It must also be noted that the NMR line corresponding to small amounts of MeOH can be broadened to beyond detection limits. After heating to 483 K DME consumption is terminated. The final products observed at this temperature are p-, o-xylenes and i-butane (24 ppm). This experiment shows clearly that DME can also serve as an alkylating agent under experimental conditions studied. 80 i-butane
xylenes .,,-,
453
,/~
60-
483 K
40
-
K toluene
DME
DME
9
Sample B
20 1:3..
298 K ,
9 '
.... ,.... ,.... ,,,35 ....,....,....,....,....,....,....,....,....,...., 65 55 25 21 ppm ,
b
I 20
~
I 40
'
I 60
'
I 80
'
10
Methanol conversion (%)
,
Figure 3. 13C MAS NMR spectra observed before and after reaction of DME and toluene over H - Z S M - 1 1 .
Figure 4. Variation of products yields as a function of methanol conversion.
To verify further whether DME is responsible for xylenes formation in course of toluene reaction with methanol, a kinetic study was performed. For that, sample C was prepared and the reaction was carried out at 433 K using the second reaction protocol (Table 1). The NMR data were then quantified, as defined in the experimental section, and product yields were plotted versus conversion to give selectivity plots [25], as shown in Fig. 4. The shapes of the selectivity patterns suggest that at low reaction temperature the major reaction pathway leading to xylenes include DME as an intermediate. On the other hand, a
33 small part of the xylene species is formed directly from methanol, as evidenced by non-zero initial selectivity to xylenes determined from the initial slope of the corresponding selectivity plot. Therefore the following reaction scheme operating in coarse of toluene alkylation is concluded: MeOH ~--- ~ DME ,~ To Iu e y "
Xylenes It should be noted, however, that contributions of these pathways to the overall xylene formation may vary with the experimental conditions (batch/flow, pressure, temperature, etc.). NMR results presented in this paper do not permit the identification of the surface active species, formed from DME and MeOH engaged in these reaction pathways and, therefore, hinder the suggestion of a more detailed reaction mechanism. The surface active species will be discussed in a further contribution [26].
3.3. Primary products of aikylation Basic principles for electrophilic substitution in the aromatic ring [27] and the extensive investigations of the electrophilic aromatic substitution in monoalkylbenzenes in homogeneous systems [28, 29] conclude to initial orto/para orientation of methyl substituent in course of toluene alkylation with methanol. When the reaction takes place on zeolite catalysts, isomerization and transalkylation reactions are usually superimposed on the primary alkylation, leading to a mixture of all xylene isomers [1-7]. In addition, product diffusion limitations within zeolite constrains may affect the ratio of xylene isomers [3, 4], preventing therefore the determination of the primary reaction products. The question of the primary products can be best answered by means of in situ techniques, which do not suffer from the above limitations. An in situ 13C MAS NMR specroscopy appears to be a suitable technique, as it allows one to distinguish unambiguously between carbon atoms of methyl groups in xylene isomers (Fig. 1). However, care should be taken while quantification of the corresponding NMR lines, as molecular dynamics of xylene isomers within zeolite pores can profoundly affect spectral features, leading to significant line broadening or even loss of intensity of one or several xylene lines. Thus, our additional experiments with the model mixtures of p- and o-xylenes adsorbed on H-ZSM-11 (not shown) indicate that a part of p-xylene molecules, corresponding to 6 molecules per u.c. of zeolite, may not be observed at room temperature, while at temperature higher than 373 K all the molecules become 'visible'. A detailed discussion of these phenomenon will be presented elsewhere [30]. For the determination of the initial ratio of the primarily formed xylene isomers, NMR experiments were performed at 387 K (Table 1, Sample D). The estimated ratio of o- and pxylenes was of two to one, indicating statistical ortho/para orientation. In conclusion, alkylation of toluene with methanol at low reaction temperatures was found to obey general concepts of electrophilic aromatic substitution [27].
4. CONCLUSIONS 1. The main reaction pathways identified in the course of methanol reaction with toluene over H-ZSM-11 under the NMRAgatch conditions are: 1) toluene methylation and 2)
34 methanol conversion to hydrocarbons followed by toluene alkylation with the fragments subsequently formed. 2 Both, methanol and dimethyl ether formed in abundance at the initial stages of reaction, may play the role of alkylating agents in toluene methylation. Under the experimental conditions studied, dimethyl ether is the main alkylating agent. 3. The primary products of toluene methylation are o- and p-xylenes, formed in the statistical ratio of two to one. ACKNOWLEDGMENTS The authors thank CICYT (project MAT 94-0359-C02-01) for financial support. I.I.I. Ivanova thanks ITQ for research postdoctoral position. REFERENCES .
2. 3. .
5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30.
N.Y. Chen, W.W. Kaeding and F.G. Dwyer, J. Am. Chem. Soc., 101 (1979) 6783. P.B. Weisz, Pure Appl. Chem., 52 (1980) 2091. W.W. Kaeding, C. Chu, L.B. Young, B. Weinstein and S.A. Butter, J. Catal., 67 (1981) 159. L.B. Young, S.A. Butter and W.W. Kaeding, J. Catal., 76 (1982) 418. J. Nunan, J. Cronin and J. Cunningham, J. Catal., 87 (1984) 77. J.-H. Kim, S. Namba and T. Yashima, Zeolites, 11 (1991) 59. K. Beschmann, L. Riekert and U. Muller, J. Catal., 145 (1994) 243. M.D. Sefcik, J. Am. Chem. Soc., 101 (1979) 2164. A. Philippou and M.W. Anderson, J. Am. Chem. Soc., 116 (1994) 5774. G. Mirth and J.A. Lercher, J. Phys. Chem., 95 (1991) 3736. G. Mirth and J.A. Lercher, J. Catal., 132 (1991) 244. G. Mirth and J.A. Lercher, J. Catal., 147 (1994) 199. E. Breitmaier and W. Volter, Carbon-13 NMR Spectroscopy, VCH Verlag, Weinheim, 1987. M.W. Anderson and J. Klinowski, J. Am. Chem. Soc., 112 (1990) 10. E.J. Munson, A.A. Kheir, N.D. Lazo and J.F. Haw, J. Phys. Chem., 96 (1992) 7740. I.I. Ivanova, D. Brunel, J.B. Nagy and E.G. Derouane, J. Mol. Catal., 95 (1995) 243. D.H. Olson and W.O. Haag, ACS Symposium Series, 248 (1984) 275. M. Guisnet and N.S. Gnep, A.S.I. Ser. E. Nato, 80 (1984) 571. A. Corma and E. Sastre, J. Catal., 129 (1991) 177. H. Vinek, M. Derewinski, G. Mirth and J.A. Lercher, Appl. Catal., 68 (1991) 277. T.R. Forester and R.F. Howe, J. Am. Chem. Soc., 109 (1987) 5076. J. Rakoczy and T. Romotowski, Zeolites, 13 (1993) 256. A. Corma, G. Sastre and P. Viruela, Stud. Surf. Sci. Catal., 84 (1994) 2171. E. Dumitriu, V. Hulea and M. Palamaru, Bul. Inst. Politch. Iasi., Sect. 2: Chim. Ing. Chim., 39 (1993) 127. A.N. Ko and B.W. Wojciechowski, Progr. React. Kinet., 12 (1983) 201. I.I. Ivanova and A. Corma, to be published. A. Schriesheim, in "Friedel-Crafts and Related Reactions", G.A. Olah (Ed.), Vol II, Interscience, New York, 1964. R.H. Allen and L.D. Yats, J. Amer. Chem. Soc., 83 (1961) 2799. M.S. Stock and H.C. Brown, Advan. Phys. Org. Chem., 1 (1963) 35. I.I. Ivanova, D. Brunel and A. Corma, to be published.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
35
S t r a t e g i e s for Zeolite S y n t h e s i s by D e s i g n M. E. Davis Chemical Engineering, California Institute of Technology, Pasadena, California 91125, United States
The thermodynamics, kinetics and a proposed synthesis mechanism for the crystallization of a prototypical high-silica zeolite, namely ZSM-5, are presented. This information is used to develop strategies for the design of zeolite syntheses and a few of these strategies are outlined. 1. I N T R O D U C T I O N
Zeolites; can they be synthesized by design? Currently, the answer to this question is no [1-3]. However, great strides are being made to reach this lofty goal of zeolite synthesis by design and I outline some of the progress below. Several factors complicate the design of zeolite synthesis. First the molecular-level of understanding of the self-assembly processes occurring during zeolite crystallizations is unknown. Second, since analogies to covalent organic synthesis [4] can not be made, the large number of organic reaction mechanisms provides little help for zeolite synthesis. With covalent organic synthesis, it is possible to systematically construct a final product by using numerous irreversible reaction steps involving different reagents and chemistries with separation between steps. Such is not the case with zeolite synthesis. With zeolites, the separation of desired from unwanted products is almost always difficult. Thus, a zeolite synthesis medium must be designed to spontaneously self-assemble into the correct architecture and atomic ordering in a single step with high yield. In view of this daunting task, the notion that zeolite syntheses can be accomplished by design has been questioned by many. I will demonstrate that this is not the case for zeolite synthesis, and that strategies for zeolite synthesis by design are currently being developed. The routes by which zeolites are crystallized from an amorphous oxide are complex and involve numerous simultaneous and interdependent equilibria and condensation steps. For this reason and others, zeolite syntheses are not well understood except that there does not appear to be a universal mechanism describing all crystallizations [1]. In this paper, emphasis ~s placed on high or pure-silica zeolite syntheses mediated by organic molecules [1,2,5]. These types of syntheses are the most amenable to design as will be described below. A typical synthesis of this kind involves the addition of water-soluble organic species into aqueous alkaline suspensions of silica. The silica dissolves and these inorganic species interact via noncovalent bonding with the organic
36 molecules to ultimately form the final organic-inorganic composite structures. The crystallization is a kinetically controlled process [1,4]. As stated above, a strategy for the design of this type of synthetic process is much different than those used in creating materials with complete covalent bonding. Whitesides et al. [4] have outlined the differences in producing new organic entities by either covalent or noncovalent synthesis. Table 1 is modified after Whitesides et al. and also contains information relevant to zeolite synthesis. The key additional factors with zeolite synthesis in comparison to totally organic preparations are the interactions between the organic and inorganic species and the condensation chemistry of the inorganic oxide. Table 1 Comparison of covalent and noncovalent syntheses (modified from ref. 4) Covalent
Noncovalent (zeolite)
Constituent bond types in the assembly process
covalent
ionic, hydrophobic, hydrogen (between organic and inorganic)
Bond strengths (kcal/mol)
25-200
0.1-5 (between organic and inorganic)
Stability of bonds in product
kinetically stable
kinetically reversible (includes silica chemistry)
Number of interactions in the assembly steps
few
many
Contributions to AG
usually dominated by AH
AH and AS can be comparable
Importance of solvent effects
secondary
primary
Other characteristics
cooperative behavior important
In this paper, I first review the salient results t h a t lead to a basic u n d e r s t a n d i n g of how high-silica zeolites are synthesized. Using this information, I then outline strategies for the synthesis of high-silica zeolites by design.
37 2. T O W A R D S A M E C H A N I S T I C U N D E R S T A N D I N G ZEOLITE SYNTHESIS
OF H I G H - S I L I C A
In the p a s t few y e a r s t h e r e has been significant a d v a n c e m e n t in the u n d e r s t a n d i n g of how the crystallization process of pure silica ZSM-5 (from now on denoted Si-ZSM-5) occurs. Here, I will use this example to highlight the g e r m a n e mechanistic issues for the synthesis of high-silica zeolites in general. In the original report on the synthesis of Si-ZSM-5, a mechanism of assembly was proposed and involved t e t r a p r o p y l a m m o n i u m cations (from now on denoted TPA) preorganizing silicate species to form the zeolite channel intersections [6]. This work and others led to the use of the term "template" to describe the role of the organic species. As pointed out by Davis and Lobo [1], the specificity between organic guest and zeolite host is as yet not sufficient to invoke true templating in the sense t h a t this term is used in biological contexts. R a t h e r we suggest t h a t the organics can act as structure-directing agents, i.e., they can dictate the final outcome of a zeolite synthesis. Figure 1 illustrates a schematic of w h a t I believe is a reasonable proposal for the TPA-mediated synthesis of Si-ZSM-5. The relevant experimental findings t h a t support this mechanistic picture are discussed below.
o
N
N. ) ~
H,
%"
H
,,I 2(" H
2
~ H " ~ I'HI
H H
Si Si
1 s
OI ~O--'Si SiI~"3"s,'Si
,,':4" ,,].w" -'-
H ~O "H 9 SO ~H
hydrophobichydration / .
.
.
.
,
,
y
i!iii:~!'ilil. ~"" :"
,
,
I
',F
J
.
o" ~ hb" T' ~ FFI~I-II ' " " "i h yorop ,,,,; .o lc ,l~-~;,i,i , ' h drat]on ~ ~ ' ' , spheres com~
,
7o~, I
,u
,
,
nucleation
70~.
,
spe~:
i
I
9
f Figure 1. Schematic Diagram of Proposed Mechanism
t agg:eW~ahibo y
38
2.1. Thermodynamics Recently, H e l m k a m p and Davis [2] have calculated e s t i m a t e s of the t h e r m o d y n a m i c p a r a m e t e r s for t h e T P A + F - m e d i a t e d s y n t h e s i s of TPAF-Si-ZSM-5 using experimental AH and AS data for quartz, amorphous silica (glass) and Si-ZSM-5 and the e x p e r i m e n t a l l y m e a s u r e d change in enthalpy for reaction (2) from Patarin et al. [7]. The synthesis of TPAF-Si-ZSM5 from quartz can be considered as follows (T=298K): quartz --~ Si-ZSM-5 AGI=AHI-(TAS)I = (5.5)-(1.4)=4.1 kJ (mol SiO2)-1
(1)
Si-ZSM-5 + TPA+F-(aq) --+ TPAF-Si-ZSM-5 + H20 AG2=AH2-(TAS)2 = (-6.2)-(1.7)=-7.9 kJ (mol SiO2)-1
(2)
quartz + TPA+F-(aq) ----> TPAF-Si-ZSM-5 + H20 AGtot=-3.8 kJ (mol SiO2)-1 When using glass instead of quartz as the starting silica, the glass-to-Si-ZSM-5 reaction yields AG3=-3.0 k J (mol SiO2) -1 and a AGtot=-10.9 k J (mol SiO2)-l. Since it is not possible to transform quartz into Si-ZSM-5, the presence of the organic structure-directing agent renders this synthesis possible (Si-ZSM-5 has been prepared from TPA and quartz [8]). For reaction (2), the favorable enthalpic term (AH_<0) is related to the van der Waals interactions between the occluded TPA molecules (or, more precisely, the TPAF ion pairs) and the SiZSM-5 framework. Additionally, there is a smaller, favorable contribution to the reaction energetics from the entropic term (TAS>0) and reflects the release of ordered water molecules from the hydrophobic hydration spheres of the TPA molecules as they are encapsulated by silicate species. TPA in Si-ZSM-5 likely represents a nearly optimum case for the organic-inorganic van der Waals interactions in zeolite synthesis. When the enthalpic contribution to AG decreases, i.e., a "looser fit" of the organic guest in the zeolite host, it is possible t h a t the entropic factor arising from the release of ordered w a t e r from the hydrophobic h y d r a t i o n sphere of the organic species m a y play a more i m p o r t a n t role in driving the s y n t h e s i s process. The observation t h a t t e t r a e t h a n o l a m m o n i u m (approximately the same size as TPA but known to not have a hydrophobic hydration sphere due to the strong hydrogen bonding with water) does not produce a zeolite product at reaction conditions where TPA would quickly yield Si-ZSM-5 supports the above statements [9]. Zones and coworkers [10,11] as well as Davis and co-workers [9,12,13] have clearly demonstrated t h a t organic species that serve as structure-directing agents in the synthesis of high-silica zeolites are intermediate in hydrophobicity. That is, m o l e c u l e s t h a t are h y d r o p h i l i c do not elicit i n t e r a c t i o n s w i t h hydrophobically hydrated silica while those that are very hydrophobic tend to aggregate and phase separate in the aqueous synthesis medium [9]. One m u s t exercise c a u t i o n w h e n a t t e m p t i n g to e x t e n d the above thermodynamic analysis of zeolite synthesis involving F- to the more standard
39 ones t h a t use OH- and/or to the addition of heteroatoms (term used here to denote non-silicon t e t r a h e d r a l atoms) such as a l u m i n u m . Pure-silica syntheses with F- can result in TPAF ion pairs being occluded in the ZSM-5 voids w i t h o u t the f o r m a t i o n of siloxy groups. W h e n using O H - a s the mineralizer, only TPA § is e n c l a t h r a t e d and the charge balance is by either Si-O- or A1-O-Si g e n e r a t e d anionic sites [14]. Thus, in order to extend the a f o r e m e n t i o n e d t h e r m o d y n a m i c a n a l y s i s to zeolite s y n t h e s i s in general, coulombic interactions m u s t be accounted for as well. Recently, Koller et al. have provided a good working model for the structure of the Si-O- site in highsilica zeolites [14]. W h a t is now needed to generalize the t h e r m o d y n a m i c analysis given above are the interaction energies between TPA and Si-ZSM-5 and TPA-ZSM-5 (contains A1) analogous to t h a t m e a s u r e d by P a t a r i n et al. [7] for TPAF-Si-ZSM-5.
2.2. Proposed Si-ZSM-5 Synthesis Mechanism A reasonable model for the m e c h a n i s m of the TPA-mediated synthesis of Si-ZSM-5 is schematically illustrated in Figure 1. Initially, the hydrophobic h y d r a t i o n sphere formed around TPA is partially or completely replaced by silicate species when a sufficient amount of soluble silicate species is available [9,12,13]. Favorable van der Waals contacts between the alkyl groups of the organic species and the hydrophobic silicate species likely provide the enthalpic driving force while the release of ordered w a t e r to the bulk aqueous phase provides an additional entropic driving force for the process [2]. It is through t h e s e o r g a n i c - i n o r g a n i c i n t e r a c t i o n s t h a t the geometric c o r r e s p o n d e n c e between the structure-directing agent and the zeolite pore architecture t h a t is the h a l l m a r k of s t r u c t u r e direction arises [1,2,8-13,15,16]. These composite species have been identified by 1H-29Si CP NMR between the protons on the TPA and the encapsulating silicates in an otherwise d e u t e r a t e d synthesis medium [12]. Additionally, silica e n c l a t h r a t e d TPA has been t r a p p e d by silylation techniques [9], and small-angle n e u t r o n s c a t t e r i n g results suggesting the p r o m p t incorporation of TPA molecules into amorphous silicate s t r u c t u r e s when TPA and soluble silicate species are mixed together [17] are consistent with this postulated first step. The availability of soluble silicates influences the r a t e at which these composite species are formed [15]. The use of a monomeric silica source such as t e t r a e t h y l o r t h o s i l i c a t e or the presence of small amounts of alkali-metal cations in the synthesis mixture t h a t facilitate the dissolution of condensed silica sources, e.g., fumed silica, colloidal silica, precipitated silica, leads to an enhanced rate of nucleation [9]. After the formation of the silica enclathrated TPA species, these composites combine to form entities of size ~ 50-70 A. These units have been identified by in situ SAXS [17,18] and cryo-TEM [19] m e a s u r e m e n t s . Additionally, units revealing the ultimate s t r u c t u r e of the final zeolite but in the size range of 80-100 A have been observed by TEM for other zeolites [20,21]. Thus, these data suggest t h a t the nucleation centers for zeolite synthesis should be smaller t h a n 100 A in size. For Si-ZSM-5, I propose t h a t the 50-70 A entities observed by various techniques are in fact the nucleation sites. These sites may form in solution (homogeneous nucleation) and/or on the reactor wall and/or on the surface of inorganic oxide particles t h a t are in the s y n t h e s i s m e d i u m ( h e t e r o g e n e o u s n u c l e a t i o n ) d e p e n d i n g upon the s t a r t i n g r e a g e n t s and synthesis conditions. Additionally, Dokter et al. suggest from in situ SAXS
40 experiments that there is an intermediate step in the formation of the 50-70 ,~ units that involves the condensation of the TPA-silicate species into aggregates by a reaction-limited cluster-cluster mechanism leading to 70 A entities with mass fractal characteristics [18]. This step makes good physical sense and is consistent with other reaction limited growth processes and nucleation activation energies not being related to diffusion but r a t h e r chemical interactions of silicate species (-90-100 kJ/mole) [15]. After the formation of the mass fractal aggregates, there is a re-organization leading to densification of the -- 70 A entities (presumably to minimize surface energies). Both the aggregation and densification processes will involve silicate bond breaking and making steps mediated by the mineralizing agent and/or alkali-metal ions. It is interesting to note t h a t for crystal nucleation from aqueous electrolyte solutions, critical nuclei sizes have been measured, are normally 2-3 unit cells and are specified as microcrsstals with the same unit cells as the final bulk crystals [22]. Thus, a 50-70 A entity of ZSM-5 would be 2-3 unit cells and this size range correlates well with other critical nuclei sizes. Dokter et al. [18] and Regev et al. [19] both suggest that after the formation of the 50-70 ,~ species, ZSM-5 crystal formation occurs via the aggregation of the 50-70 /~ entities. Alternatively, we have proposed that the surfaces of the 50-70 A nuclei serve to "template" the crystal growth process by using the enclathrated TPA species as building units. Thus, the growth occurs in a layer-by-layer fashion [12,13]. Although aggregation of the 50-70 A entities into larger structures has been suggested from SAXS data, this crystal growth mechanism can not account for the layer-by-layer growth that is necessary for the formation of ZSM-5/ZSM-11 intergrowths [23] and could only occur with homogeneous nucleation. Thus, we suggest that crystal growth can occur in a layer-by-layer fashion [12,13]. This proposal for crystal growth may be more generally applicable to zeolite synthesis since layer-by-layer crystal growth is also implied by the intergrowth structures of zeolite beta [24], SSZ-26/SSZ33/CIT-1 [25-28], FAU/EMT [29-30], OFF/ERI [31], MAZ/MOR [31] and other non-zeolitic, crystalline oxides [32]. In fact, we have shown with two distinctly different zeolite systems, i.e., FAU/EMT [30] and SSZ-33/CIT-1 [27,28], that the control of the layer stacking sequence can be performed in a systematic and designed fashion t h r o u g h the purposeful m a n i p u l a t i o n of the organic structure-directing agents. If a layer-by-layer growth mechanism is feasible, then two questions immediately arise: (i) is the layer-by-layer growth truly single layer additions or are the building entities larger? and (ii) do the composite organic-inorganic species function as the building entities or do organic molecules adsorb onto the growing crystal surface from solution and then organize inorganic building units? To answer the first question, the upper bound on the number of layers possible in the growth step will be the minimum size of the observed stacking units in the crystal. Recently, Pan and co-workers have shown via high-resolution TEM images that the minimum size of stacking units can in fact be one layer for the n a t u r a l zeolite tschernichite (analogue of zeolite beta) [33]. Thus, single layer building units are possible. The answer to the second question is less clear. Vaughan has proposed that inorganic cations, e.g., Na § K § play a role in determining the s t r u c t u r e of the inorganic building units while the organics function to influence the orientation in which these structures assemble to create the longrange order [20]. For aluminosilicate materials like FAU/EMT where Si/A1
41 3.5-5.0, this type of mechanism appears plausible [29]. Recently, Stevens and Cox postulated a similar growth mechanism for zeolite beta by proposing that the organic molecules adsorb onto the growing crystal surface [34]. Since two equi-energetic orientations were possible, and since polymorphs A and B are postulated to have the same lattice energy [35], a high degree of faulting was predicted [34] (as is experimentally observed [24,33]). For high- and/or puresilica compositions it is hard to imagine otherwise that at least a portion of the units necessary for crystal growth would have to be silicate enclathrated organic species. These species are necessary for the formation of nuclei and it is most likely that they also participate in the growth process. Twomey et al. have shown that when Si-ZSM-5 is removed from its crystallization medium, nucleation and growth can be restarted [15]. These authors suggest that organic-inorganic entities are continually being produced and upon formation have to choose between nucleating new crystals or incorporating into those that already exist and are growing. From the experimentally measured crystal size distributions, Twomey et al. suggest that incorporation and growth are favored under typical conditions [15]. These results are consistent with silicate enclathrated organic species acting as building entities for crystal growth. However, these building units may be used in combination with "free" organic molecules that adsorb on the crystal surfaces and also participate in concert in the growth process. Evidence to support this conjecture is that ZSM-5 can be synthesized with occluded tetramethylammonium cations (TMA has been shown to not be enclathrated by silicate species [12 ]) if the synthesis mixture contains a sufficient amount of TPA (in addition to TMA) to induce nucleation and sustain crystal growth (Si/TPA=17; TPA/TMA>l)[36]. Thus, if this mechanism is close to the true molecular level assembly process then structure-direction appears to critically influence the ultimate fate of the crystallization at the nucleation stage. 2.3. K i n e t i c s
Since the kinetics of nucleation are typically slower than the kinetics of crystal growth in high- and/or pure-silica syntheses, the kinetics of nucleation play a significant role in determining the phase produced. Goepper et al. have shown that alkali-metal cations influence the rate of nucleation and crystal growth of pure-silica zeolites [37]. Additionally, Burkett and Davis have observed an isotope effect in pure-silica syntheses in the presence and absence of alkali-metal cations [9]. Pure-silica zeolites crystallize faster in H20 than D20 at low alkali-metal ion concentrations. This result supports the premise that O - - H (O--D) bond breaking is also important to zeolite crystallizations. With higher alkali-metal ion concentrations and/or the use of monomeric silica sources, the crystallization proceeds rapidly and the isotope effect becomes less obvious [9]. If the alkali-metal ion concentration is large, these cations compete with the organic species for interactions with the silicate species and ultimately form layered products [38]. This behavior can be rationalized using the bond valence approach of Brown [39]. That is, the best valence match with sodium ions is silicate ions that give layered structures rather than tectosilicates [39]. Since the nucleation step is typically the rate limiting process in highand/or pure-silica zeolite syntheses, the Ostwald ripening model would predict that increasing crystallization rates should be observed with increasing
42 stability of the crystallization material [8]. Recently, Harris and co-workers have shown that rate of crystallization (rate determining step is nucleation in this case) of nonasil does in fact increase as the calculated stabilization energy increases as predicted by the Ostwald ripening model [40]. It is suggested that as the organic molecular size more closely matches the nonasil cage size that there is an increase in van der Waals interactions t h a t lead to the energetic stabilization [40] (recall thermodynamic a r g u m e n t s described previously for TPAF-Si-ZSM-5). The one exception to the trend reported by Harris and coworkers was t h a t the largest organic molecule used (should have had the tightest fit according to the model calculations) had a slow crystallization rate. F u r t h e r work is necessary in order to u n d e r s t a n d this single anomalous experiment. 3. STRATEGIES F O R SYNTHESIS BY D E S I G N
If the thermodynamic, kinetic and mechanistic descriptions of high-silica syntheses of zeolites described above are phenomenologically correct, then this information can be used to develop strategies for zeolite synthesis by design. Two aspects of the design process are described below: (i) the design of pore architectures and (ii) the design of framework atom positioning. In order to develop a zeolite pore architecture by design, the proper choice of organic structure-directing agent and inorganic composition m u s t be made. The organic molecule m u s t have intermediate hydrophobicity and be able to organize w a t e r molecules as has been described by Zones, Davis and coworkers [9-13]. Next, the size and rigidity of the molecule m u s t be controlled. It is clear t h a t as the size of the organic molecule is increased, the specificity for producing zeolite pore architectures also increases [10]. Very recently, Zones has shown t h a t there is a good correlation between structure direction and the rigidity of the organic structure-directing agent as m e a s u r e d by the number of tertiary and quaternary connectivities in the molecule for a series of organics with C/N§ [11]. Thus, size, rigidity and hydrophobicity s i m u l t a n e o u s l y m u s t be correctly specified in order to p r e p a r e a good structure-directing agent by design. For the inorganic compositions, it is clear t h a t for pure-silica preparations a small a m o u n t of alkali-metal cations is necessary for practical kinetics [37]; however, large a m o u n t s will lead to layered compounds [2,38,39]. Since the Si-O-Si angle can vary greatly with little difference in energy [41], it is not surprising t h a t the enthalpies of formation for numerous pure-silica zeolites are all within 2RT (twice the thermal energy) at typical synthesis conditions [42]. Thus, numerous pure-silica structures are energetically feasible and the choice of the product formed is made by the kinetic p a t h w a y specified by the organic s t r u c t u r e - d i r e c t i n g agent. If heteroatoms, e.g., A1, B, Zn, are added into the inorganic mixture, they can strongly influence the s t r u c t u r e s produced even in a m o u n t s as small as SIO2/M203 = 50 [4,10]. We ascribe this behavior at least in part to the loss of flexibility in the Si-O-M angle as compared to the Si-O-Si bonding [4,10,11]. The loss of energetically feasible angles with the addition of heteroatoms creates a reduction in the possible atomic a r r a n g e m e n t s when compared to pure-silica structures. One fairly clear consequence of heteroatom addition is the shift from u n i d i m e n s i o n a l pore s y s t e m s (highly p r o b a b l e w i t h p u r e - s i l i c a
43 compositions) to multidimensional pore architectures [10]. A stellar example of the design of a zeolite pore architectural is by Zones in the synthesis of SSZ-26 [43]. Zones et al. prepared a polycyclic, rigid, diquaternary structure-directing agent to synthesize a multidimensional, large pore zeolite. Using this structure-directing agent and a low-alkali-metal cation c o n t a i n i n g a l u m i n o s i l i c a t e r e a c t i o n composition, a new multidimensional large-pore zeolite was synthesized [25,26,43]. This is the first example of a zeolite with a new pore architecture that was crystallized by the purposeful design of the structure-directing agent. For certain applications of zeolites, e.g., catalysis, it could be important to be able to place particular atoms into specific framework positions by design. Based on the aforementioned mechanism of high-silica zeolite crystallization, Li et al. synthesized ZSM-5 and ZSM-5/ll intergrowths using an organic structure-directing agent that contained a covalently attached silicon atom in order to test whether the silicon atom linked to the organic could be incorporated into a framework position [44]. Li et al. successfully implanted the silicon atom into a framework position as verified by solid-state NMR experiments. Thus, a strategy for designing atomic arrangements is now available in the attachment of target atoms onto specified positions of the organic structure-directing agent [44]. Currently, a completely designed synthesis of a zeolite has not been accomplished. However, the future is bright in this area. The design of structure-directing agents and synthesis compositions is occurring. A more complete design in the sense of the entire framework structure and atom positionings will require f u r t h e r molecular-level insights into the crystallization mechanism. RE~~CES 1. 2. 3. 4. 5. 6. 7. 8. ,
10. 11. 12. 13.
R.F. Lobo and M.E. Davis, Chem. Mater., 4 (1992) 756. M.M. Helmkamp and M.E. Davis, Annu. Rev. Mater. Sci., 25 (1995) 161. M.E. Davis, CHEMTECH, Sept. (1994) 22. G.M. Whitesides, E.E. Simanek, J.P. Mathias, C.T. Seta, D.N. Chin, M. Mammen and D.M. Gordon, Acc. Chem. Res., 28 (1995) 37. B.M. Lok, T.R. Cannan and C.A. Messina, Zeolites, 3 (1983) 282. E.M. Flanigen, J.M. Bennett, R.W. Grose, J.P. Cohen, R.L. Patton, R.M. Kirchner and J.V. Smith, Nature, 271 (1978) 512. J. Patarin, H. Kessler, M. Soulard and J.L. Guth, ACS Symp. Ser., 398 (1989) 221. R.A. van Santen, J. Keijsper, G. Ooms and A.G.T.G. Kortbeek, Stud. Sur. Sci. Catal., 28 (1986) 169. S.L. Burkett and M.E. Davis, Chem. Mater., submitted. R.F. Lobo, S.I. Zones and M.E. Davis, J. Incl. Phenom., in press. S.I. Zones and M.E. Davis, in Synth. Microporous Materials: Zeolites, Clays, Nanocomposites, (eds.) M. Occelli and H. Kessler, Marcel Dekker, NY, in press. S.L. Burkett and M.E. Davis, J. Phys. Chem., 98 (1994) 4647. S.L. Burkett and M.E. Davis, Chem. Mater., in press.
44 14. 15. 16. 17. 18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30. 31. 32. 33. 34. 35. 36.
37. 38. 39. 40. 41. 42. 43. 44.
84
H. Koller, R.F. Lobo, S.L. Burkett and M.E. Davis, J. P h y s . Chem., submitted. T.A.M. Twomey, M. Mackay, H.P.C.E. Kuipers and R.W. Thompson, Zeolites, 14 (1994) 162. H. Gies and B. Marler, Zeolites, 12 (1992) 42. L.E. Iton, F. Trouw, T.O. Brun, J.E. Epperson, J.W. White and S.J. Henderson, Langmuir, 8 (1992) 1045. W.H. Dokter, H.F. Van Garderen, T.P.M. Beelen, R.A. van Santen and W. Bras, Angew. Chem. Int. Ed. Engl. 34 (1995) 73. O. Regev, Y. Cohen, E. Kahet and Y. Talmon, Zeolites, 14 (1994) 314. D.E.W. Vaughan, Stud. Sur. Sci. Catal., 65 (1991) 275. M. Tsapatsis, T. Okubo, M. Lovallo, and M.E. Davis, MRS Symp. Ser., in press. I.N. Tang and H.R. Munkelwitz, J. Coll. Inter. Sci., 98 (1984) 430. G.R. Millward, S. Ramdas, J.M. Thomas and M.T. Barlow, J. Chem. Soc., Faraday Trans., 79 (1983) 1075. M.M.J. Treacy and J.M. Newsam, Nature, 332 (1988) 249. R.F. Lobo, M. Pan, I. Chan, H.X. Li, R.C. Medrud, S.I. Zones, P.A. Crozier and M.E. Davis, Science, 262 (1993) 1543. R.F. Lobo, M. Pan, I. Chan, R.C. Medrud, S.I. Zones, P.A. Crozier and M.E. Davis, J. Phys. Chem., 98 (1994) 12040. R.F. Lobo, S.I. Zones and M.E. Davis, Stud. Sur. Sci. Catal., 84 (1994) 461. R.F. Lobo and M.E. Davis, J. Am. Chem. Soc., 117 (1995) 3766. S.L. Burkett and M.E. Davis, Microporous Mater., 1 (1993) 265. J.P. Arhancet and M:E. Davis, Chem. Mater., 3 (1991) 567. D.E.W. Vaughan in Multifunctional Mesoporous Inorganic Solids, (eds.) C.A.C. Sequeira, M.J. Hudson, Elsevier, Amsterdam (1993) 137. C.N.R. Rao and J.M. Thomas, Acc. Chem. Res., 18 (1985) 113. R. Szostak, M. Pan and K.P. Lillerud, J. Phys. Chem., 99 (1995) 2104. A.P. Stevens and P.A. Cox, J. Chem. Soc., Chem. Commun. (1995) 343. S.M. Tomlinson, R.A. Jackson and C.R.A. Catlow, J. Chem. Soc., Chem. Commun. (1990) 813. J.A. Rossin and M.E. Davis, Ind. J. Technol., 25 (1987) 621. M. Goepper, H.X. Li and M.E. Davis, J. Chem. Soc., Chem. Commun. (1992) 1665. S.I. Zones, Microporous Mater., 2 (1994) 281. I.D. Brown, in Structure and Bonding in Crystals, (eds.) M. O'Keefe and A. Navrotsky, Academic Press, NY (1981) 1. T.V. Harris and S.I. Zones, Stud. Sur. Sci. Catal., 84 (1994) 29. M.D. Newton and G.V. Gibbs, Phys. Chem. Miner., 6 (1980) 305. I. Petrovic, A. Navrotsky, M.E. Davis and S.I. Zones, Chem. Mater., 5 (1993) 1805. S.I. Zones, M.N. Olmstead and D.S. Santilli, J. Am. Chem. Soc., 164 (1992) 4195. H.X. Li, M.A. Camblor and M.E. Davis, Microporous Mater., 3 (1994) 117.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
45
Use of Modified Zeolites as Reagents Influencing Nucleation in Zeolite Synthesis s. I. Zones and Y. Nakagawa Chevron Research and Technology Company Richmond, California 94802-0627 USA 1. INTRODUCTION New molecular sieve structures continue to be generated and the majority of these reactions rely on the participation of an organic component which is often found within the crystallized inorganic host lattice. There continues to be much debate regarding the role of various types of organic components in the crystallization process. Are there structure-directing roles that these organics fulfill in such areas as forming nuclei, redistributing solubilized silicate populations, aiding in crystal growing, or a number of other critical functions during the synthesis which are difficult to measure experimentally [ 1]? One of the more important results to impact this area of research has been the finding of Navrotsky and co-workers that the novel silicate zeolite structures formed in the presence of organic components do not differ much from each other in enthalpy of formation [2,3]. The enthalpy values are also not far removed from either very dense phases or amorphous silicates. A model of a guest/host complex that resides in an energy well as compared to a non-ordered gel state, while attractive in explaining the important role of the organics in zeolite synthesis, is not well supported by this calorimetry research. In fact, an energy balanced calculation for the formation of TPA*F-/MFI from quartz suggests that the entropic contributions may be the most important factors to consider in the crystallization process [4]. The burden of explaining the effectiveness of the organic reagents then shifts to the issue of zeolite synthesis kinetics and nucleation events. One of our recent studies addressed nucleation selectivity as related to a "goodness-of-fit" for nuclei which resemble the final crystalline product [5,6]. Bell and Chang also developed a model of zeolite crystallization from clathrated organic guests [7]. In this study we wish to continue this discussion on nucleation rate and phase selectivities in the presence of organic structure-directing agents, but with the focus on using highly porous zeolites as inorganic reactants. We have demonstrated that FAU materials are interesting reagents for delivery of A1 to a synthesis gel [8], and similarly, boron-beta zeolite has proven to be an even more impressive reagent for crystallizing novel borosilicate sieves [9]. We have expanded upon this work by modifying some of these reagents and examining the effects of modification of these reagents.
2. EXPERIMENTAL Two types of zeolite synthesis reactions were studied. In the first type, reactions were performed using calcined boron-beta zeolite as borosilicate source [ 10], a quaternary ammonium hydroxide compound, sodium hydroxide, water, and additional boron from sodium borate
46 decahydrate. In the second type of reaction, Cabosil M5 or "N" silicate was mixed into a solution of the two bases mentioned above and aluminum was provided as FAU zeolite [ 11 ], which in most instances was modified by ion-exchange with a transition metal. Care was taken to monitor the pH of the exchange to avoid precipitation from the hydrolysis of the hydrated cation. Table 1 describes the reactant ratios and reaction conditions used in the synthesis studies. The quaternary ammonium compounds used in this study are illustrated in Table 2. The zeolite synthesis reactions were run in Teflon cups for 23 mL Parr stainless steel reactors, and were heated with or without tumbling in Blue M convection ovens [ 12]. Crystallized products were analyzed by X-ray diffraction on a Siemens D-500 instrument. Elemental analyses were determined by ICP methods at Galbraith Laboratories, Knoxville, Tennessee (U.S.A.). Table 1 Reaction Conditions for Molecular Sieve Synthesis Reaction Type Conditions
Borosilicate
High OH A1
Low OH A1
OH/SiO2
0.25
0.90
0.30
Na/Si
0.10
0.90
0.12
Organic/Si
0.15
0.08
0.18
A1/Si
0.00
0.07
0.07
B/Si
0.05-0.10
0.00
0.00
H20/Si
44
32
28
Temp., ~
150
135
160
0
43
43
2-4
2-8
6-9
rpm Time, Days
Table 2 Organocations Used in the Study
Structure
Code
.3)~
T06
+
(CH3)3N~ (CH3)~
T20 ~1CH313
F40
Structure
Code B100
~ 3 I§ CH 3 ~
~
Me 3
M46
~ ~ F~1CH313 B15
B08 N(CH3)3
47
3. RESULTS AND DISCUSSION 3.1. Studies with boron-beta zeolite In our previous study we demonstrated that calcined boron-beta zeolite had limited stability under hydrothermal conditions and as such, could be converted to other zeolites in the presence of certain organocations [9]. Use of this reagent led to rapid nucleation in synthesis reactions, reducing crystallization times to a matter of hours as compared to weeks for synthesis of some zeolites, such as SSZ-24. No amorphous phase intermediate is detected in these conversion reactions. In fact, if the boron-beta alone is heated long enough in water, thereby becoming mostly amorphous, when it is used as a synthesis reagent, the rate and phase selectivity features are lost [13]. The reaction selectivity can sometimes be changed in the presence of additional borate. This demonstrates an interesting synergy between dissolved borate or borosilicates and the high surface area borosilicate zeolite. Is the re-dissolution of the boron-beta an important step in the rapid nucleation? Since borate has high solubility in basic solution, the role of the extra borate added may be to shift the equilibrium toward species which are needed in the synthesis of zeolites such as SSZ33, which appear to require some amount of lattice substitution in order to form [ 13]. We know that the boron-beta zeolite must eventually break down as part of the reaction process because products such as SSZ-24, which contain only 4- or 6-ring subunits, are obtained. The starting boron-beta zeolite contains 5-rings as well, therefore we do not believe that the conversions are a result of "local" transformations involving existing subunits at the surface of the beta-zeolite. Table 3 shows the results of conversion experiments run with and without extra borate. The most spectacular result is the shift in product from SSZ-24 to SSZ-33 upon changing the borate concentration in the presence of organocation T20. SSZ-24 is a large-pore, one dimensional zeolite, whereas SSZ-33 has a multidimensional, 12-10 pore system. F40, which was used to discover SSZ-26 [15] will make SSZ-33 provided there is sufficient boron available in the conversion reaction. Use of boron-beta zeolite is critical in this conversion, as evidenced by the failure of F40 to form SSZ-33 if more conventional, soluble sources of silica and boron are used. The organocation used by Lobo and Davis to discover CIT-1 (B 15) can affect, to some degree, conversion of boron-beta zeolite to CIT- 1, the pure polymorph B of the mixture which constitutes SSZ-33 [16]. B08, the organocation which crystallizes SSZ-33 from soluble systems, does not convert boron-beta into the expected product. We were at first surprised by the lack of reactivity observed in this reaction. Table 3 Conversion of Boron-Beta to Other Organo-Zeolites Organocation
Product
Product (B4Q'/Added)
T06
SSZ-24
SSZ-13
T20
SSZ-24
SSZ-33
F40
SSZ-33
SSZ-33
B08
Beta
Beta
B 100
SSZ-35
SSZ-35
B 15
CIT- 1/Beta
M46
Beta
Beta
48 Recently we showed that the boron-beta product from the reaction with B08 is not strictly "unreacted" [ 13]. We found that the pore system of the product was filled with B08 and that this was true even if the reaction was carried out at 85~ Our interpretation is that the organocation rapidly fills the beta pore system before nucleation to other structures can begin. We believe that the availability of the zeolite reactant surface is an important part of this transformation synthesis. This is similar to our earlier observations that FAU is not a viable reactant in zeolite synthesis if the pore access is blocked [ 11 ]. In Table 2, the entry M46 is similar in size to the adamantyl or tricyclodecane templates, but M46 is structurally much more flexible. As such, it very effectively inhibits conversion of boron-beta to other phases. In fact, using a mixed template system where one component is M46, all conversions were inhibited with the exception of the M46/TPA system, where we did observe formation of ZSM-5. Since calcined boron-beta zeolite has such attractive properties (enhanced rates, novel products) as a reagent for molecular sieve synthesis, we wondered if there were any other zeolites which would also behave in this capacity. Since we believe that high surface area materials are desirable, multidimensional materials would be the first likely candidates. We therefore considered using borosilicates SSZ-33 and B-ZSM-5. Neither of these materials show any reactivity in comparable conversion reactions. Part of the problem may be due to the stability of these zeolites under hydrothermal conditions. Both calcined SSZ-33 and B-ZSM-5 were found to be stable to prolonged aqueous heating, and are extremely steam stable. This again supports the hypothesis that the boron-beta zeolite breaks down under the reaction conditions prior to recrystallization of the new phase. 3.2. Reactions with modified Y zeolite (FAU) A number of years ago Bourgogne, Guth, and Wey demonstrated that Y zeolite can be used as an aluminum source in reactions to crystallize ZSM-5 [ 17]. More recently, we showed that Y zeolite can be used to prepare novel materials such as Al-rich beta which is difficult to make by other routes [ 18]. Other novel materials become accessible by using a very high Si/A1 version ofY [ 19]. Might the selectivity be changed further in our zeolite synthesis reactions if we ion-exchanged the Na in the Y zeolite for metals which would not easily re-exchange back out in basic solution? To test this, we prepared a series of ion-exchanged modified Y zeolites which are shown in Table 4. We envisioned that the rate of delivery of A1 (as AI(OH)4 or A1-O-Si-O units) might be slowed due to the blockage caused at the site by the potentially insoluble hydrolyzed metal. Table 4 Ion-Exchanged FAU as Reagent in Zeolite Synthesis Metal
% Exchange for Na
Solution pH
Surface Area m2_/g
Fe III (b)
80
2.10
346
Cr Ill (b)
75
3.10
532
Co II (c)
64
7.35
674
Ni (b)
69
6.60
664
Ag (b)
65
6.80
Zn (c)
71
6.40
600
Cu II (b)
75
4.38
656
(a) Exchange carried out at 23~ for 16 hours with M+z/A1 set at 5 for z=3 and 7.5 for z=2. (b) Nitrate salt (c) Acetate salt
49 Figure 1 shows a kinetic profile of crystallization of SSZ-13 (CHA) from T06 using the exchanged Y zeolites. We have shown that for this "high OH" type reaction (see Table 1), the pH increase above the buffering capacity of silicate is a good measure of extent of crystallization [8,11 ]. In this reaction the adamantyl organocation is found inside the chabazite cages and typical product SiO2/A1203 values are 10-12. 13.00 -
(~
.-.--~ ............
~_____.
,,~......................
,|
/
/ / ... / / /
I
lZSO-
_-
,' .~.~-
t
' ----'~
.....
~> .....
@--
*
iI / 12.00
-
@
~
@
~
~
To Point
_ _ ' " ' " ~ - ~ " " " ' " ' . ". . .". . ~. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
"@
,
0
25
50
75
100 200
Hours at 135~
Figure 1. Conversion of metal-exchanged Y zeolites (see Table 4) to SSZ-13. Rates are determined by pH increase during crystallization. The hydrothermal crystallization uses organocation T06 from Table 2 and "high OH" conditions in Table 1. Typically, no crystallization begins before about 10 hours and pH values remain at T o, the value before heating. Three groups of kinetic response were observed. Relative to the control (Na-Y), Co-Y or Cu-Y reaction rates were just as fast, indicating no retardation of crystallization. A second group consisting of Ni-Y, Ag-Y, and Zn-Y showed a slower growth rate. Here the pH-profile suggests that nucleation is not retarded, but that the overall crystallization is slower. These metals may affect the availability of A1 in solution. It is unclear as to why the Ag reactions plateau at a lower final pH. Fe and Cr, two trivalent metals, when exchanged into Y zeolite, completely inhibit the reaction! No transformation is observed, even at 200 hours ofreaction time. This may in part be due to the reduced surface areas for these latter two reagents (Table 4). Fe-Y shows the largest decrease of the prepared materials, and the fact that it has also lost 60% of its available micropore volume suggests that Fe has precipitated in the pores. In Table 1, a set of aluminosilicate reactant conditions at "low OH" is described. These conditions were used successfully in the synthesis of SSZ-26 [20], and the products of this type of reaction typically have SiO2/A1203 of 20-30. The reactant SiO2/A1203value is 35 (using Y zeolite with a value of 5 as a reagent), which is still in a range where SSZ-13 can be made from the adamantyl-type cations. We have shown that as the SiO2/A1203 reactant values change using T06, a progression of SSZ-13 (highest [A1]), SSZ-23, and SSZ-24 (lowest [A1]) can be produced [21].
50
In the same study it was pointed out that the use of methylene blue dye appeared to suppress the crystallization of SSZ-13 and allowed us to crystallize pure aluminosilicate SSZ-23. SSZ-23 is a novel (unsolved) structure which we believe has a constrained 10-ring pore system with sizable cavities (to accommodate the adamantyl cations) and higher surface area than other known intermediate pore zeolites (near 500 m2/g). If Co-Y is used under the "low OH" conditions, a Co-containing SSZ-13 is crystallized. However, if Cr-Y is used, Cr-SSZ-23 is crystallized in a region which would normally produce SSZ- 13 ! Based on the results in Table 1, we would not have expected to see any conversion at all. Therefore, in both "high" and"low" OH-type experiments, Cr-Y appears to be an inhibitor for SSZ13 formation (although the mechanism of inhibition might not be the same in the two reaction types). Since we were curious about how much of an inhibitory effect the Cr-Y had in these types of reactions, we ran a series of reactions where varying amounts of both Cr-Y and Co-Y were used as a source of aluminum. The results are graphed in Figure 2 and three product regions emerge. 0.80
0.70
0.60
0.50
| ~" 0.40 0 (.) 0.30
0.20
SSZ-24 Region
|
0.10 , 00
0.10
gi~ I
0.20
0.30
0.40
Cr+31AI
Figure 2. Zeolite synthesis from Co and Cr-exchanged Y zeolite as A1 source and under "low OH" conditions (Table 1). The amount of Co and Cr are inversely adjusted in the experiments and the mixture of zeolite products recovered is plotted. Organocation used was T20 (Table 2). SSZ- 13 (CHA) forms only in the presence of very minor amounts of Cr-Y; chromium seems to be a very effective inhibitor of its crystallization. When Co-Y is the major contributor, surprisingly, SSZ-24 forms. In this instance, the combined Co-Y and Cr-Y do not participate in the reaction; the SSZ-24 is crystallizing from the silica, added alkali and organocation. The metalexchanged Y materials are uninvolved "spectators" and FAU is detected in the isolated solids. (In an analogous experiment, this same behavior was observed for template B08 producing SSZ-31 and unreacted metal-Y). As Cr-Y becomes the major A1 source, SSZ-23 progressively dominates over SSZ-24 as the crystallization product. However, this SSZ-23 zeolite product contains both the chromium and aluminum from the starting reagent.
51 In the "high OH" reaction Cr-Y gave no product. The Cr-Y inhibits SSZ- 13 formation which needs some A1 to nucleate and grow, but the OH/Si level in these experiments is too high to nucleate all-Si SSZ-23 [22]. Under the "low OH" conditions, the SSZ-13 inhibition remains but SSZ-23 crystallizes. The fascinating change here is that the nucleation of SSZ-23 is not likely to be an allSi event favorable at these OH/Si ratios because SSZ-24 would be the more likely crystallization product. Therefore, relatively low amounts of A1 must be available at this early stage and by the end of the reaction, all of the Cr-Y is consumed, (only SSZ-23 is seen in the XRD), and A1 is transferred into the new structure. Catalytic activity is seen for the (chromium) aluminosilicate product, indicating incorporation of A1 into framework positions. Chromium is found associated with the SSZ-23 which is also recovered as a green solid! We do not have evidence at this time indicating the location of the chromium in the product, and there is no reason to believe that it is a framework component or in cationic sites in the organo-zeolite. 4. CONCLUSIONS Highly porous zeolites such as FAU and boron-beta are useful reagents for delivering A1 and B to growing organosilicate lattices during synthesis. The high surface areas of these reagents allow for rapid interaction with the synthesis solution providing for attractive nucleation rates. The way in which components are delivered to the nucleation site (by an unknown mechanism) can also alter the phase selectivity in the experiment. By ion-exchanging the FAU with transition metals whose hydrolysis products have limited solubility in basic solutions, the synthesis selectivity is altered even further. 23 Cr-Y was found to be a good inhibitor for SSZ-13 crystallization in the presence of adamantyl derivatives. The A1 could, however, be eventually transported into a growing SSZ-23 structure. This approach in zeolite synthesis may hold further promise for generating novel structures, compositions, or controlled lattice substitution in zeolite synthesis products. ACKNOWLEDGMENTS
We thank Lun Teh Yuen and Greg S. Lee for synthesis of organocations and help in running the zeolite syntheses. Chevron Research is gratefully thanked for permission to present this work and for continued research support. REFERENCES
1. 2. 3. 4. 5.
6. 7. 8. 9.
M.E. Davis, Chemtech (Sept. 1994), 22. I. Petrovic, A. Navrotsky, S. I. Zones, and M. E. Davis, Chem. Mater. 5 (1993) 1805. N.J. Henson, A. K. Cheetham, and J. D. Gale, Chem. Mater. 6 (1994). M.M. Helmkamp and M. E. Davis, Ann. Rev. Mater. Sci. (1995 in press). T.V. Harris and S. I. Zones, "Zeolites and Related Microporous Materials: State of the Art 1994," Ed. J. Weitkamp, H. G. Karge, H. Pfeifer, W. Holderich, (Elsevier, Amsterdam) (1994) 29. M.E. Davis and S. I. Zones, Third International Symp. on Synthesis of Microporous and Layered Mater. Ed. M. L. Occelli, H. Kessler in press. C.D. Chang and A. T. Bell, Catal. Lett. 8 (1991) 305. S.I. Zones, J. Chem. Soc. Farad. Trans. 86 (1990) 3467. S.I.Zones, L. T. Yuen, Y.Nakagawa, R.A. VanNordstrand, andS.D. Toto, inProc. 9thlnt'l. Zeol. Conf., Ed. R. von Ballmoos, J. B. Higgins, M. M. Treacy (Butterworth-Heinemann, Stoneham, Massachusetts) (1993) 163.
52 10. S.I. Zones, L. T. Yuen, and S. D. Toto, U.S. Patent 5,187,132 (1993). 11. S.I. Zones, J. Chem. Soc. Farad. Trans. 87 (1991) 3709. 12. Y. Nakagawa and S. I. Zones, "Molecular Sieves, Synthesis of Microporous Materials, Vol. 1," Ed. M. L. Occelli, H. E. Robson (Van Nostrand-Reinhold, New York) (1992) 222. 13. S.I. Zones and Y. Nakagawa, Microporous Mater 2 (1994) 543. 14. R.F. Lobo, M. Pan, I. Y. Chan, R. C. Medrud, S. I. Zones, P. A. Crozier, and M. E. Davis, J. Phys. Chem. 98 (1994) 12040. 15. S.I. Zones, M. M. Olmstead, and D. S. Santilli, J. Amer. Chem. Soc. 114 (1992) 4195. 16. R.F. Lobo, S. I. Zones, and M. E. Davis, "Zeolites and RelatedMicroporous Materials: State of the Art 1994," Ed. J. Weitkamp, H. G. Karge, H. Pfeifer, W. Holderich (Elsevier, Amsterdam) (1994) 461. 17. M. Bourgogne, G. L. Guth, and R. Wey, U.S. Patent 4,503,024 (1985). 18. S.I. Zones and Y. Nakagawa, U.S. Patent 5,340,563 (1994). 19. S.I. Zones and Y. Nakagawa, U.S. Patent 5,225,179 (1993). 20. S.I. Zones and D. S. Santilli, Proc. 9th Int'l. Zeol. Conf., Ed. R. von Ballmoos, J. B. Higgins, M. M. Treacy (Butterworth-Heinemann, Stoneham, Massachusetts) (1993) 171. 21. S. I. Zones, R. A. VanNordstrand, D. S. Santilli, D. M. Wilson, L. T. Yuen, and L. D. Scampavia, "Zeolites: Facts, Figures, Future, "Ed. P. A. Jacobs, R. A. vanSanten (Elsevier, Amsterdam) (1989) 299. 22. S.I. Zones, European Patent 213,018 (1987). 23. We have found that the ion-exchange properties of boron-beta zeolite are not as straightforward and hope to report on these findings in the near future.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
53
Templating Studies Using 3,7-Diazabicyclo[3.3.1]nonane Derivatives: Discovery of New Large-Pore Zeolite SSZ-35 Y. Nakagawa Chevron Research and Technology Company Richmond, California 94802-0627 USA In our continuing studies of rigid, polycyclic organocations as structure-directing agents for zeolite synthesis, we have focused on the 3,7-diazabicyclo[3.3.1]nonane skeleton. Various derivatives of this family can be used as templates in zeolite synthesis reactions, leading to the formation of large-pore zeolites. For example, the N,N,N'-trimethyl-diazabicyclononane derivative, A, results in crystallization of the novel zeolite, SSZ-35, over a broad range of inorganic reaction conditions. We believe that SSZ-35 is a multi-dimensional zeolite possessing at least one 12-ring channel system. Larger derivatives of A resulted in the crystallization of unidimensional large-pore zeolite, SSZ-24. 1. INTRODUCTION Many of the recent discoveries of new high-silica zeolitic frameworks have been achieved through the use of novel organocationic templates as structure-directing agents. Large-pore, unidimensional zeolite SSZ-24 (AFI-type) was first discovered by Zones using trimethylammoniumsubstituted adamantanes. ~ This was followed by the discovery of large-pore multi-dimensional zeolite SSZ-26, which was made using a rationally designed propellane-based template. 2-4 ZSM18 was first discovered using an unusual tris-pyrrolidinium cation. 5,6 The success of this approach has encouraged us to search for new organic structure-directing agents which we hope will lead to the discovery of new zeolitic structures. We have reported on the use of Diels-Alder chemistry to efficiently prepare a series of structurally related polycyclic organic templates which were effective in crystallizing zeolites ZSM-12, SSZ-31, SSZ-33 and SSZ-37. 7,8 In this study, three large organic templating agents based on a 3,7-diazabicyclo[3.3.1 ]nonane skeleton were synthesized and their effectiveness as structure-directing agents were explored. One derivative in particular, Template A, has led to the discovery of a new multi-dimensional zeolite, S 5 Z - 3 5 . 9
2. EXPERIMENTAL Template Synthesis: Templates A and B were synthesized using the double-Mannich reactions described in references 9 through 11. Methylamine hydrochloride was heated in the presence of glacial acetic acid and paraformaldehyde, and the resultant mixture was added to the appropriately N-substituted 4-piperidone. After purification by extraction and fractional vacuum distillation, the intermediate 9-keto-3,7-diazabicyclononane was subjected to Wolff-Kishner reduction in a mixture of hydrazine, potassium hydroxide and triethylene glycol. The resulting 3,7-diazabicyclononane was treated with methyl iodide to afford the corresponding quaternary ammonium iodide salt, which was recrystallized prior to ion-exchange.
54 Sparteine-derived Template C was prepared by neutralization of commercially available (-)-sparteine sulfate pentahydrate (Aldrich) using aqueous NaOH, followed by extraction into dichloromethane. 12,13 The free diamine was quarternized in chloroform using methyl iodide, and the resulting mono-methylated salt was recrystallized from a mixture of acetone and diethyl ether with a small amount of added methanol. The iodide salts wer~ converted into the hydroxide form by ion-exchange using Bio-Rad AG lX8 (20-50 mesh, hydroxide form) in a minimum amount of water. The molarity of the resulting template solutions was determined by titration using phenolphthalein as an indicator.
Zeolite Synthesis: Zeolite synthesis reactions were performed in 23 mL Teflon cups for Parr 4745 reactors and were heated in Blue M ovens as previously described. 8 Reagents and ratios for the various synthesis reactions will be described in more detail in following sections. Products were analyzed by X-ray diffraction using a Siemens Model D500 diffractometer (using CuK ). SEM micrographs were taken on a Hitachi S-570 instrument. Elemental analyses of solids were performed at Galbraith Laboratories using ICP methods. C and N levels were determined on a Carlo Erba unit.
Template Structures: CH3
CH3~ N + ~ I
~N~ X-
CH 3
N~
CH3 CH3 ~ .N+ / CH 3
A
XB
CH3 CH3
N
X
C
3. RESULTS AND DISCUSSION Our previous studies using rigid, polycyclic organocations derived from Diels-Alder chemistry demonstrated their effectiveness in directing toward crystallization of interesting large-pore molecular sieves. 7,8 These studies also illustrated how other factors greatly affect the observed product selectivity: a given template may give rise to several different products depending on the starting gel composition. The three new templates discussed in this study were designed to capture similar space-filling characteristics of the successful Diels-Alder templates. We chose a large carbon skeleton to ensure that the organocations would not make clathrasil-type structures, and also incorporated two nitrogens in the template, thus keeping the C/N ratio within a reasonable range (< 8), in order to retain its water solubility.
3.1. SSZ-35 Zeolite Synthesis We were gratified to discover that the first template we synthesized, Template A, did in fact lead to the crystallization of a novel new phase, SSZ-35. SSZ-35 can be prepared under a variety of conditions to afford purely siliceous SSZ-35, as well as boro- and aluminosilicate compositions. This is in contrast with the tricyclo-undecene Template (D) from our Diels-Alder series which gave three different zeolites (SSZ-31, SSZ-33 and SSZ-37) from three different gel compositions) The selectivity for making SSZ-35 is quite high for Template A, and the framework structure of SSZ35 apparently tolerates the levels and types of substitution observed. Under more traditional high
55
aluminum and alkali hydroxide conditions (A1/Si = 0.06; NaOH/Si = 0.055), the frequently encountered SSZ- 13 (CHA) phase was obtained. Typical reaction conditions for the synthesis of SSZ-35 are given in Table 1. 9'14 Table 1 Reaction Conditions for Synthesis of SSZ-35 Using Template A
SiO2/W203 oo 50 33 100 50
W
A/Si
M+/Si
OH/Si
B B A1 A1
0.20 0.22 0.33 0.20 0.20
0.05 0.08 0.04 0.05 0.05
0.25 0.25 0.33 0.25 0.25
Temperature 160~ 160~ 160~ 170~ 170~
M=Na, K Silica sources include Cabosil M-5 fumed silica and Ludox AS-30 colloidal silica. Boron sources include Na2B4OT10H20 and boric acid; Reheis F2000 dried aluminum hydroxide gel was used as a source of aluminum. Typical H20/Si ratios were from 35-50. Reaction times ranged from 10-12 days, however, by seeding the reaction mixture with as little as 0.5 wt % SSZ-35 crystals, complete crystallization could be achieved in 5 days. A typical preparation of borosilicate SSZ-35 is described below: Template A (3.2 grams of a 0.70 M solution), 3.3 g water, and 0.45 mL of 1.0 N NaOH were added to a 23-mL Teflon cup of a Parr 4745 reactor. Sodium borate decahydrate (0.045 g) was added and the mixture was stirred until homogeneous. Ludox AS-30 (DuPont, 1.36 g) was added to give a starting gel with a SiOJB203 of 28. The reaction was heated at 160~ (static) for 12 days, after which the settled solid was collected and washed thoroughly. XRD indicated that the product was SSZ-35, and the product was found to have a SiO2]B203 of 53. Characterization The XRD patterns for both as-made and calcined all-silica SSZ-35 are shown in Figure 1. The material is stable to calcination in air to 595~ and the distinctive pattern is not reminiscent of any previously-reported zeolites, therefore we believe that SSZ-35 represents a new framework topology. Unit cell parameters and symmetry for calcined SSZ-35 were determined from synchrotron data: ~5
Symmetry:
triclinic _a = b = c =
13.9719(24) * 18.1747(28) 7.3734(16)
alpha beta gamma
= = =
90.87 ~ 98.93 ~ 90.55 ~
Scanning electron micrographs for all-silica and aluminosilicate SSZ-35 are shown in Figure 2. The difference in crystal size due to introduction of aluminum into the framework is readily apparent.
56
'
"
'
'
'
,
,
,
I
....
9
,
Calcined SSZ-35
rl r
I-- O ~
;~"
uJ t.z
III
-----.._~
o
~_~
7'.2
xb.4
tb.6
~.a
2b.o
TWO -
THETA
2w
2~.4
~.e
3~,.e
36.0
9(DEGREES)
As-made SSZ-35
,i Q.
z
uJ i-.
o
~
q
32B
t
TWO
-
THETA
{OEGREES)
Figure 1. Powder XRD Patterns of As-made and Calcined SSZ-35
360
57
~3CMASNMR spectra confirmed that Template A was still intact within the channels of SSZ35. Weight losses of 13-17 wt % were observed above 250~ using TGA on the as-made product. For one-dimensional large-pore zeolites such as SSZ-24 and ZSM-12, weight losses above 250~ are typically 10-11 wt %; therefore, we anticipated that there would be a large void volume in the SSZ-35 framework. The BET area for SSZ-35 was found to be -- 500 m2/g and adsorption data (shown in Table 2) are comparable to other multi-dimensional frameworks with different dimensionalities. H-SSZ-35 was shown to have a Constraint Index ~6 of < 0.8, indicative of the structure having at least one large-pore channel system. Table 2 Adsorption Data for SSZ-35 (in cc/g; P/P Q = 0.15) Zeolite
N2
n-hexane
cyclohexane
SSZ-35 Beta SSZ-24 ZSM-5 SSZ-37
0.20 0.26 0.12 0.14 0.18
0.15 0.24 0.10 0.14 0.16
0.09 0.25 0.12 0.04 0.14
a) All-Silica SSZ-35
Channel system
3D; 1D; 3D; 2D;
? 12R x 12R 12R 10R x 10R 10R x 12R
b) Aluminosilicate SSZ-35 (SiO2/A1203 = 65)
Figure 2. Scanning Electron Micrographs of All-Silica and Aluminosilicate SSZ-35
58
3.2 Related Templates While the N,N,N'-trimethyl-3,7-diazabicyclo[3.3.1]nonane Template A is very selective for new zeolite SSZ-35, the corresponding N'-isopropyl derivative, Template B, exhibits a high selectivity for the SSZ-24 framework (although in an all-silica reaction, both SSZ-31 and SSZ-24 are seen as products). The even larger methyl sparteine derivative (Template C) also strongly directs toward SSZ-24 crystallization. Representative results using this family of templates are shown in Table 3. Table 3 Results of Various Screening Reactions using 3,7-Diazabicyclononanes
Template A B C
Reaction Type Boron-Containingt
All-Silica SSZ-35 SSZ-31 +/or SSZ-24 SSZ-24
Aluminum-Containingw
SSZ-35 SSZ-24 SSZ-24
SSZ-35 SSZ-24 + Layered SSZ-24
t Starting SiO2/B203 = 33 - 50 (Cabosil/Na2B407 or H3BO3; B-beta zeolite) w Starting SiO2/A1203 > 200 (Cabosil/Reheis F200; Tosoh Y390 high silica FAU) The observation that these larger templates resulted in the formation of a one-dimensional zeolite was somewhat surprising at first. We originally thought that larger templates were better candidates for crystallizing multi-dimensional zeolites. In trying to understand why only Template D gave SSZ-37, while other closely related analogs do not, we have learned from modeling studies that it is extremely important to consider how the templates occupy the channel system. 7 In the case of SSZ-37, two template molecules can effectively fill the interconnecting 12-ring channel system. 17 If the template is any larger, two molecules no longer fit within the defined space, and one template alone cannot provide sufficient stabilization of the channel. Although we have not yet determined the structure of SSZ-35, it is possible that Templates B and C (and even only slightly larger N-Me,N-ethyl derivative E) fail to give SSZ-35 for the same reason. If the length ('T': see Figure 3) of a structure-directing agent is too great, one-dimensional zeolites are formed. We have observed this tendency with several of our"linear" templates where the observed product is ZSM12,18 and Casci has reported similar results using bis-trimethyl ammonium templating agents. ~9 In the latter case, the "default" products are medium-pore zeolites EU-2 (ZSM-48) and ZSM-23, whose channel systems are complementary to the width and height of the bisquat salts. ~ N ~ CH3
//_ H3C ~ CH3 O
I+ CH3 X-
CH3
E
59 1 v
Figure 3. Important Dimensions of Structure-Directing Agents The dimensions of the 3,7-diazabiocyclononane templates (calculated h -- 7.5 ]k; w -- 5.0/~k) 20 are too large to be accommodated in ZSM-12 channels (MTW pore dimensions: 6.2 x 5.5 x 5.2 A), but they fill the SSZ-24 pore system (d = 7.5 A) optimally. In fact, the selectivity for making SSZ24 using Templates B and C is so high that we are able to prepare B-SSZ-24 directly from Cabosil and soluble sources of boron (Na2B407 or H3BO3),rather than having to start with calcined B-beta as described in Zones' earlier work using trimethylammonium adamantane derivatives. ~2,2~ Davis and Lobo observed the same phenomenon, which they attributed to the hydrophobicity of the methyl sparteine template. 13,22,23Although hydrophobicity may be a contributing factor, our belief is that direct synthesis of B-SSZ-24 is possible because the diazabicyclononane derivatives B and C prevent the formation of a cage-type structure such as SSZ-13 (CHA), which is the favored product from the adamantyl derivatives as lattice substitution is introduced. Although the charged nitrogen to carbon ratio of the methyl sparteine template is high, the presence of the second nitrogen in the molecule reduces the overall C/N to 8, thereby making it less hydrophobic. We have also been able to incorporate a small amount of aluminum directly into the SSZ-24 structure using Template C and Cabosil and Reheis F2000 aluminum hydroxide dried gel to give a product with a final SiO2/A1203 of 270. In addition, from a high silica Y-zeolite (Tosoh Y390) as a starting source of both silica and alumina, 24we obtained an SSZ-24 product with a SiOJA120 3 of 400. Although we have demonstrated that it is possible to prepare A1-SSZ-24 directly using Template C, the level of aluminum incorporation which is possible is still quite low. Aluminum exchange of B-SSZ-24 as described by Zones et al. still affords a more highly substituted aluminum-containing product. 25 4. CONCLUSIONS A new zeolite, SSZ-35, was discovered using the 3,7-diazabicyclo[3.3.1 ]nonane Template A. This zeolite can be prepared over a range of compositions and appears to possess a multidimensional channel system having at least one large-pore component. Related Templates B and C do not lead to the crystallization of this new phase, but rather, exhibit a selectivity for SSZ-24. We believe that these results can be explained by the inability of the 12-ring component of the SSZ35 structure to accommodate the larger Templates B and C. These templates therefore induce the formation of one-dimensional, large-pore zeolites such as SSZ-31 or SSZ-24. B-SSZ-24 can be made directly from soluble reagents using these templates, and does not require the use of calcined B-beta zeolite as a starting material. When substituting elements are introduced into the starting gel, products such as CHA often are favored, however, the steric requirements of Templates B and C are such that they cannot be accommodated within the CHA cage. Thus, the direct systhesis of B-and A1-SSZ-24 becomes possible.
60 ACKNOWLEDGMENTS
We thank Gregory S. Lee for synthesizing the organic templates described in this study and for assistance in running the zeolite screening reactions, R. A. Van Nordstrand for preliminary XRD work and Dr. R. C. Medmd, Dr. G. Zhang and G. Mondo in collecting the synchrotron data on SSZ-35. We also acknowledge the work of Dr. Medmd in determining the symmetry and unit cell parameters for both as-made and calcined SSZ-35. Dr. T. V. Harris provided assistance in modeling of the templates and Dr. S. I. Zones was involved in many helpful discussions. We also thank Chevron Research and Technology Company for continuing support of this program and permission to publish this work. REFERENCES
1. 2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21.
22. 23. 24. 25.
S.I. Zones, U.S. Patent No. 4 665 110 (1987). S.I. Zones, U.S. Patent No. 4 493 337 (1990). S.I. Zones, U.S. Patent No. 4 190 006 (1990). S.I. Zones, M. M. Olmstead, D. S. Santilli, J. Am. Chem. Soc., 114 (1992) 4195. S.L. Lawton, W. J. Rohrbaugh, Science, 247 (1990) 1319. J. Ciric, U.S. Patent No. 3 950 496 (1976). Y. Nakagawa, Studies in Surface Science and Catalysis, J. Weitkamp, H. G. Karge, H. Pfeifer, W. Holderich, eds., Part A, Elsevier (1994) 323. Y. Nakagawa, S. I. Zones, "Synthesis of Microporous Materials, Vol. 1," M. L. Occelli and H. Robson, eds., Van Nostrand Reinhold (1992) 222. Y. Nakagawa, U.S. Patent No. 5 316 753 (1994). S.A. Zisman, K. D. Berlin, F. K. Alavi, S. Sangiah, C. R. Clarke, B. J. Scherlag, J. Of Labeled Compounds and Radiopharmaceuticals, 27 (1989) 885. S.A. Zisman, K. D. Berlin, B. J. Scherlag, Org. Prep. and Proc. Int., 22 (199) 255. Y. Nakagawa, U. S. Patent No. 5 271 922 (1993). R.F. Lobo, M. E. Davis, Microporous Materials, 3 (1994) 61. We have since found other templates which make SSZ-35 and have broadened the synthesis ranges described in this paper: Y. Nakagawa, U.S. Patent No. 5 268 161 (1993) Y. Nakagawa, U.S. Patent No. 5 273 736 (1993). Synchrotron data was collected on X7A beam line, National Synchrotron Light Source, Brookhaven National Laboratory, which is supported by the U. S. Department of Energy, Division of Materials Sciences and Division of Chemical Sciences. V.J. Frilette, W. O. Haag, R. M. Lago, J. Catal., 67 (1981) 218. J.L. Casci, M. D. Shannon, P. A. Cox, S. J. Andrews, "Synthesis of Microporous Materials, Vol. 1," M. L. Occelli, H. Robson, eds., Van Nostrand Reinhold (1992) 359. S.I. Zones, Y. Nakagawa, J. W. Rosenthal, "Zeolites (Japan)," 11 (1994) 81. J.L. Casci, New Developments in Zeolite Science and Technology, Y. Murakami, A. Iijima and J. W. Ward, eds., Elsevier (1986) 215. Molecular dimensions were calculated using "Smallest cylinder program" which was developed at Chevron Research and Technology Co. by Paul Merz. S.I. Zones, L-T. Yuen, Y. Nakagawa, R. A. Van Nordstrand, S. D. Toto, "Proceedings from the Ninth International Zeolite Conference," R. Von Ballmoos, J. B. Higgins and M. M. J. Treacy, eds., Vol. 1, Van Nostrand Reinhold (1993)163. R. de Ruiter, J. C. Jansen, H. Van Bekkum, Zeolites, 12 (1992) 56. Although Davis and Lobo did not observe conversion of calcined B-beta zeolite to B-SSZ24 using Template C, we did obtain B-SSZ-24 from B-beta after 7 days at 150~ S.I. Zones, Y. Nakagawa, U. S. Patent No. 5 225 179 (1993). R.A. Van Nordstrand, D. S. Santilli, S. I. Zones, "Synthesis of Microporous Materials, Vol. 1," M. L. Occelli and H. Robson, eds., Van Nostrand Reinhold (1992) 373.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
61
S y n t h e s i s of Z S M - 4 8 T y p e Zeolite in P r e s e n c e of Li, Na, K , R b and Cs Cations G. Giordano 1, A. Katovic 1, A. Fonseca 2 and J.B. Nagy 2 1Dipartimento di Ingegneria Chimica e dei Materiali, Universit~t della Calabria, 1-87030 RENDE (CS), Italy 2Laboratoire de Catalyse, Facult6s Universitaires Notre-Dame de la Paix, 61 rue de Bruxelles, B-5000 NAMUR, Belgium
SUMMARY
This study investigates the formation of ZSM-48 zeolite starting from a hydrogel with or without A1 as a function of the alkali cations (Li, Na, K, Rb and Cs). Crystallization kinetics data, chemical composition, NMR characterization, morphology and crystal size are presented in order to give additional information about the synthesis of this catalyst precursor. INTRODUCTION Recently, the preparation of ZSM-48 type zeolite has shown a new interest due to its catalytic properties as additive in FCC catalyst. The presence of ZSM-48 in FCC catalyst increases both conversion and selectivity in C3-C 4 products [1]. The ZSM-48 possesses a 10MR unidimensional channel system with pore opening 5.3 x 5.6 A and it can be synthesized starting from silica or alumino-silicate gels in presence of various organic compounds. The nature of inorganic and organic cations affects the formation of ZSM-48 and also influences morphology, crystal size and the amount of structural defects. The aim of this work is to evaluate the effect that the alkaline cations (Li, Na, K, Rb and Cs) have on the synthesis of ZSM-48 zeolite in a system that contains hexamethonium ions (HM++). ~ The data about crystallization kinetics, morphology, crystal size, chemical analysis and NMR characterization are discussed with the goal to optimize the synthesis of ZSM-48 in HM systems. EXPERIMENTAL The synthesis was carried out at 200~ under static condition and autogenous pressure in Teflon-lined Morey-type autoclaves starting from the following hydrogel: 5 M20 - 2.5 HMBr 2 - x A1203 - 60 S i t 2 - 3000 H20 where HMBr stands for hexamethonium bromide, x = 0 or 0.5 and M = Li, Na, K, Rb or Cs. The samples were filtered, washed, dried and characterized by usual procedures (X-ray, SEM, EDX, A.A. spectroscopy and NMR).
62 RESULTS AND DISCUSSION
First of all, it can be observed that in absence of A1 the systems with Li, Na and K show similar crystallization kinetics. After 24 hours of reaction the crystallinity is higher than 90%. In presence of Rb ions a reaction time of about 48 hours is required for a complete crystallization. The Cs ions disfavour the formation of ZSM-48, since the first crystals are detected, by X-ray, only after 30 hours while with the other cations the crystallization is almost complete at that time. Moreover, the maximum of crystallinity (60%) is obtained after 50 hours of reaction, and at longer times co-crystallization with cristobalite occurs. The presence of A1 in the starting hydrogel leads to a longer crystallization time. Similar behaviour is observed for other zeolites such as the MFI type. In this case all the inorganic cations, except Cs ions, show similar behavior. In fact the nucleation time is identical for all four samples and after 48 hours of reaction all samples show more than 85% crystallinity. Also in this case, the presence of Cs ions disfavours the ZSM-48 formation. Indeed, after 4 days of reaction the crystallinity achieved is only 35%. However, in this case the formation of cristobalite is not observed for longer reaction times. Chemical analyses show that the amount of HM ions is close to one per unit cell for all examined samples. In the synthesis in absence of A1, only traces of alkaline cations are detected. This suggests that the synthesis of the siliceous ZSM-48 can be obtained also in absence of inorganic cations, and hence only a component is required that solubilizes and mobilizes the siliceous species. On the other hand, the amount of organic cations detected is justified by the large amount of structural defect observed by 29Si-NMR analysis. In the samples synthesized in presence of A1, both inorganic and organic cations are found in the final products. The amount of inorganic cation observed is not sufficient to act as counteractions of A1 species, and this suggests that also the hexamethonium ions play a role in stabilizing the negative charges. Probably the organic cations stabilize the framework by a pore filling action and act as neutralizing agent of the negative charges and of the defect groups. The number of A1 per unit cell found in the final products is always less than 1, and this is in agreement with the framework suggested for the ZSM-48 zeolite. In fact when the amount of A1 in the initial reaction mixture increases, the system derives toward the formation of EUO type zeolite. The 27A1-NMR data show that the aluminium is incorporated in the ZSM-48 zeolite mainly in the tetrahedral coordination. The spectra of 29Si-NMR show that the amount of SiOM (M = organic and/or alkali cation) defect groups is higher in absence than in presence of A1. Indeed, in presence of Li, Na, K and Rb, some 18 SiOM/u.c. are detected without A1, and ca 12 SiOM/u.c. with A1 incorporated in the structure. These values are higher than those reported previously in the presence of Na and a high amount of HM §247ions [2]. In presence of Cs, the amount of SiOM/u.c. is smaller (13/u.c.) and the 29Si-NMR spectrum shows a higher resolution. REFERENCES 1. F. Di Renzo, G. Giordano, F. Fajula, P. Schultz and D. Anglerot, French Pat. 2.698,863 (1994). 2. G. Giordano, N. Dewaele, Z. Gabelica, J.B. Nagy, A. Nastro, R. Aiello and E.G. Derouane, Stud. Surf. Sci. Catal., 69 (1991) 157.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
63
O u t - o f - p l a n e B e n d i n g Vibrations of Bridging OH G r o u p s in Zeolites: A New Characteristic of the G e o m e t r y and Acidity of a B r o e n s t e d Site L.M. Kustov*, E. Loeffler**, V.L. Zholobenko*, and V.B. Kazansky* *N.D. Zelinsky Institute of Organic Chemistry, Russian Academy of Sciences, Moscow, Leninsky prosp. 47, 117334 Russia **Adlershofer Umweldschudztechnik, Berlin, Rudower Chaussee 5, D-0-1199 Germany
Abstract Out-of-plane bending vibrations of bridging OH groups in zeolites were studied by diffuse-reflectance IR spectroscopy in the region of the combination bands of the out-of-plane bending and fundamental stretching vibrations (3800 - 4200 cm -1). Similar to the in-plane bending vibrations, the out-of-plane bending modes were found to be a very sensitive characteristic of the bridging OH groups in zeolites. These frequencies increase with increasing acidity of the OH groups and with formation of H-complexes with adsorbed molecules.
1. INTRODUCTION The observation of the bending, torsional, and other low-frequency vibrations of the structural hydroxyl groups in oxide adsorbents and catalysts encounters a number of problems because of the unfavorable background due to the framework vibrations in the region of 200 - 1000 cm-1, as well as due to the low concentration of OH groups. There are however two possible ways to overcome this difficulty: (i) the use of modern highly sensitive spectroscopic methods for studying OH groups, for instance, Fouriertransform IR, diffuse-reflectance IR, inelastic neutron scattering, etc. and (ii) the analysis of the combination bands. In our previous studies [1 - 3], we have analyzed the combination modes (v + (3) of the fundamental stretching and in-plane bending vibrations in the DRIR spectra of zeolites and other oxide materials using highly sensitive diffuse-reflectance IR spectroscopy. The bending vibrations of the bridging
64 OH groups were shown to be much more sensitive to the structural environment of hydroxyls as compared to the stretching vibrations. Thus, two types of the isolated bridging hydroxyl groups characterized by the frequency of the fundamental stretching vibration at 3660 cm -1 have been resolved in the region of the combination bands of the stretching and in-plane bending vibrations. The range of the stretching frequencies for various types of OH groups is quite narrow (3550 - 3800 cm -1), i.e., about 250 cm -1, whereas the corresponding range of the in-plane frequencies is much wider and extends from 600 cm-1 (for MeOH groups connected with rare-earth cations) to 1640 cm -1 (for water molecule). The in-plane bending frequencies were also proposed as an additional measure of the acidic properties of these OH groups. In studying structural OH groups in SAPOs [4], we succeeded in observing a combination band of the fundamental stretching and out-of-plane bending vibrations of the bridging OH groups. The combination band for SAPO-34 was found at 3940 cm -1, which was attributed to the structural OH groups characterized by the fundamental stretching frequency at 3600 cm -1 Thus, the out-of-plane bending frequency calculated as the difference of the two observed frequencies is equal to 340 cm-1. The quantum-chemical calculations [5, 6] agree fairly well with the experimental data and show that the bending modes are more sensitive to changes in the local structure at the Broensted site compared to the stretching modes. The calculations allowed the authors to estimate the outof-plane bending frequency for the bridging OH groups in zeolites (y - 400 cm-1). Recently, the fundamental in-plane bending and out-of-plane bending modes for the bridging OH groups in zeolites have been observed using inelastic neutron scattering spectroscopy at 1090 cm-1 and 420 cm-1, respectively [ 7 - 11], in perfect agreement with the theoretical prediction and our studies of the combination bands. In the present paper, we attempted to use the similar approach to investigate the combination bands of the stretching and out-of-plane bending vibrations of structural OH groups in different types of zeolites.
2. E X P E R I M E N T A L H-forms of the zeolites X (Si/AI = 1.25), Y (Si/AI = 2.35), erionite (Si/AI 3.5), mordenite (Si/AI = 21) and ZSM-5 (Si/AI = 21) were prepared by calcination of ammonium forms in a vacuum at 640 - 770 K depending on the thermal stability of the zeolites. The thermal-vacuum pretreatment at the final temperature was performed for 8 h, The rate of the temperature increase was 2 - 5 K/min. The diffuse-reflectance IR spectra were measured using a Perkin-Elmer 580B spectrophotometer as described in [1, 2]. Adsorption of N20, CO 2, n-
65 C8F18, and CF3H was carried out at room temperature pressures of 20 - 40 torr.
and adsorbate
3. R E S U L T S A N D D I S C U S S I O N DRIR spectra of the HNaY, HNaX, and HNa-ERI zeolites under study in the region of 3200 - 4000 cm -1 are presented in Fig. 1. The absorption bands in the region of 3550 - 3750 cm -1 have been reliably assigned to the fundamental stretching vibrations of the bridging hydroxyl groups [1, 2, 12]. However, in some cases, additional low-intensity lines at 3900 - 3950 cm-1 are also observed. These bands are present in the spectra of H-forms of X and Y zeolites and erionite, but they are absent in the spectra of the HZSM-5 zeolite and H-mordenite. Although X, Y, and erionite zeolites have so little in common as concern their structure, stability, and chemical composition, it is still possible to find at least one common feature distinguishing them from pentasils. Indeed, the socalled LF-bands in the low-frequency region (3520 - 3580 cm-1) are observed in the IR spectra of X, Y, and erionite zeolites. They have been attributed to the bridging OH groups, which are hydrogen-bonded to the neighboring oxygen atoms of the lattice in the double 6-membered rings (D6R structural elements) [1, 12]. For the pentasil-type zeolites, such as mordenite and ZSM5 zeolite, this type of H-bonding is not realized because of the absence of the D6R units in the structures of these zeolites. Hence, an assumption could be drawn that the bands near 3900 cm-1 are observed only in those cases when the bands at 3520 - 3580 cm-1 are present in the IR spectra. To confirm this hypothesis, HX and HY zeolites with different ion-exchange degree of Na + for NH4 -I- (o~) were investigated. As is seen in Fig. l b, for faujasites with 0c < 50%, unlike the samples with 0c > 70%, the intensity of the band at 3550 - 3580 cm-1 is much lower than that of the band at 3650 cm-1 Accordingly, the intensity of the high-frequency band at 3900 cm-1 decreases in a similar way. Thus, these data show that the band at 3900 - 3950 cm-1 is somehow connected with the bridging OH groups that are H-bonded to the oxygen atoms of the lattice in the D6R structural units (vOH - 3520 - 3580 cm-1). The high values of the frequencies corresponding to the observed maxima (-3900 cm-1), which are placed far beyond the region of the stretching vibrations of OH groups and the significant halfwidths of the bands (AH1/2=80 - 100 cm -1) allow us to assign them to a combination v + ~/, i.e., to a combination of the stretching vibration ( v ) o f the H-bonded acidic hydroxyl groups with a low-frequency vibration ~f. The y values derived by subtraction of the stretching frequency from the combination are presented in Table 1. They are ranged from 325 to 380 cm-1 depending on the zeolite. In our opinion,
66 3610
3640
3560 1 1
3555 ~~ 3660
,/ _,j! 3,<,s .J
.',
2
1
I
3580
tt, l // ///
\.j~ /
I 3740
//
/ / f 2 / /
/
I / ~
J
3928
Fig. 1. DRIR spectra of H-forms of zeolites in the region 3300 - 4000 cm-1 (a) HZSM-5 (1), H-MOR (2), and H-ERI (3) (b) HNaX (1), HNaY-45% (2), and HNaY-80% (3).
6?
Table 1 Spectroscopic parameters of the bridging OH groups forming a hydrogen bond with framework oxygen atoms in zeolites.
Zeolite
HNaX HNaY H-ERI
v, cm -1
3580 3555 3560
v +~/, cm -1
3905 3928 3940
T, cm -1
325 373 380
Table 2 Spectroscopic parameters of bridging OH groups in the HZSM-5 zeolite forming a hydrogen bond with adsorbed molecules.
Adsorbate
v, cm- 1
v + y, cm- 1
y, cm- 1
CF3H
3530
3910
380
CO 2 N20
3470 3450
3940 3925
470 475
68
this vibration should be classified as an out-of-plane bending vibration of hydrogen bonded OH groups in the bridging fragment: ~Si
mI
" ~ ' 0 ..--H ..... 0 .~AI ~ " Indeed, the frequencies of the in-plane bending vibrations of OH groups (6) are known to be about of 800 - 1100 cm -1 and corresponding combination modes are ranged from 4500 to 4700 cm -1 [1 - 3]. The frequencies of the out-of-plane bending vibrations of isolated OH groups in alcohols are reported to be 200 - 220 cm -1 [13]. When H-bonding takes place, the frequency increases to 300 - 400 cm -1, in parallel with strengthening of an H-bond [13]. Consequently, the v + 3' combination band for the isolated acidic OH groups (vOH = 3610 - 3660 cm -1) , which should have the frequency at 3800 - 3850 cm -1 seems to be hardly observed on the background caused by the absorbance of silanol groups (VOH = 3740 cm-1). An increase in the frequency of the out-of-plane bending vibration for Hbonded OH groups with the enhancement of their acid strength may be explained by the fact that the O - H " ' O fragment becomes more rigid. It should be also noted that for X and Y zeolites having identical structures, the y values are quite different. Moreover, in the HY zeolite, which is more acidic than the HX zeolite, OH groups are characterized by a larger y-frequency shift as compared with its assumed value for isolated OH groups ( ~ / - 200 - 220 cm-1). This is in agreement with the above-mentioned dependence found for alcohols [13] more acidic hydroxyls that form stronger hydrogen bonds, exhibit higher values of the y frequency. Thus, the frequency of the out-of-plane bending vibration of the bridging OH groups may be used as an additional measure of their acidic properties. In the case of H-erionite, an increase in the frequency of the out-of-plane bending vibration as compared with faujasites is observed as well. However, this comparison seems to be incorrect, because the structures of erionite and faujasites are quite different and, consequently, the O ...... O distances in the O--H...O fragments may be changed. From the data obtained, it is possible to suppose that the band at 3900 3950 cm-1 may be observed even for the zeolites, which do not contain structural elements of the D6R type, if their acidic OH groups form H-bonds with adsorbed molecules. This hypothesis is confirmed by our data on N20, CO 2, n-C8F18, and CF3H adsorption on the HZSM-5 zeolite. Admission of these adsorbates leads to the formation of weak hydrogen bonds with the bridging OH groups (z~v = 60 - 150 cm-1). The adsorption results also in the appearance of the low-intensity absorption bands at 3910 - 3940 cm -1 in the IR spectra (Fig. 2). The calculated frequencies of the bending vibrations (Y)in
d9
3470 3450
1
q
3530
d
4
4 , / /
3610
/
3700
".X/~
9
, /
/
,/
/ 1
~
.j" ! [ 3745 ~"l
J
I
2
', \
A,
1
3925 "\ 3910 o
q I ~3940
I I ', \ \\
Fig. 2. DRIR spectra of the HZSM-5 zeolite before (1) and after adsorption of trifluoromethane (2), nitrous oxide (3), and carbon dioxide (4) at room temperature.
70 accordance with the above hypothesis increase with a strengthening of an Hbond (see Table 1). Thus, the bands at 3900 - 3950 cm-1 revealed in IR spectra of zeolites should be attributed to the combination modes (v + T) of the stretching and out-of-plane bending vibrations of the bridging OH groups forming hydrogen bonds with lattice oxygen atoms. These frequencies could be used to calculate the frequency T of the out-of-plane bending vibrations. The data on the T frequencies seem to give an additional information about acidic properties of the OH groups and about the geometric characteristics of the hydrogen-bonded complexes.
REFERENCES 1. L. M. Kustov, V. Yu. Borovkov, and V. B. Kazansky, J. Catal., 72 (1981) 149. 2. V. B. Kazansky, L. M. Kustov, and V. Yu. Borovkov, Izv. Chim. Bulg. Akad. Nauk, 16 (1983) 44. 3. L. M. Kustov, V. Yu. Borovkov, and V. B. Kazansky, Zh. Fiz. Khim. (Russ. J. Phys. Chem.), 59 (1985) 2213. 4. S. A. Zubkov, L. M. Kustov, V. B. Kazansky, et al., J. Chem. Soc., Faraday Trans., (1991) 897. 5. J. Sauer, J. Mol. Catal., 54 (1989) 312. 6. J. Sauer, Chem. Rev., 89 (1989) 199. 7. M. J. Wax, R. R. Cavanagh, J. J. Rush, et al., J. Phys. Chem., 90 (1986) 532. 8. T. J. Udovic, R. R. Cavanagh, J. J. Rush, et al., J. Phys. Chem., 91 (1987) 5968. 9. H. Jobic, J. Catal., 131 (1991) 289. 10. W. P. J. H. Jacobs, H. Jobic, J. H. M. C. van Wolput, and R. A. van Santen, Zeolites, 12 (1992) 315. 11. W. P. J. H. Jacobs, J. H. M. C. van Wolput, R. A. van Santen, and H. Jobic, Zeolites, 14 (1994) 117. 12. J. W. Ward, In: Zeolite Chemistry and Catalysis, (J. A. Rabo, Ed.), ACS Monograph 171, American Chemical Society, Washington D.C., 1976. 13. J. Rossarie, J.-P. Gallas, C. Binet, and R. Romanet, J. Chim. phys. phys.chim. biol., 74 (1977) 202.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviotand S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
71
In situ F T I R microscopic investigation of the acid sites in cloverite G. MOiler, G. Eder-Mirth and J.A. Lercher Christian Doppler Laboratory for Heterogeneous Catalysis and University of Twente, Department of Chemical Technology, P.O. Box 217, 7500 AE Enschede, The Netherlands. The acidity of cloverite was studied by sorption of probe molecules with varying basicity. Cloverite possesses two types of structural hydroxyl groups (Ga-OH and P-OH groups) which exhibit high and moderate Br6nsted acid strength towards apolar hydrocarbon molecules. Sorption of polar base molecules on the Ga-OH groups, however, leads to a breaking of the GaO bond close to the Ga-OH adsorption site resulting in a concerted Lewis and Br6nsted type interaction. For small molecules (like ammonia), multiple sorption at these sites causes a local rearrangement of the lattice leading to a collapse of the microporous structure upon thermal desorption of the probe molecules. Small alcohols are chemisorbed quite differently on the Ga-OH groups of cloverite compared to other acidic molecular sieves leading to the formation of dimethylether and formaldehyde upon desorption. 1. INTRODUCTION Cloverite, a microporous gallophosphate has attracted great attention as it possesses unusually large micropores [ 1-3]. Because of its potential as sorbent and catalyst for the reactions of larger organic molecules, the structure was thoroughly characterized by various techniques [ 17]. A major drawback for its application, however, is the instability of the microporous structure in ambient atmosphere once the template is removed. This is also the main reason why rather limited information is available on the sorption and catalytic properties of the molecular sieve [ 14,6]. The aim of this contribution is to characterize the nature and strength of the acid sites of cloverite by sorption and reactive desorption of probe molecules. The molecules studied were the strong bases ammonia, pyridine and trimethylamine as well as alcohols with varying chain length (methanol, ethanol and propanol). 2. EXPERIMENTAL 2.2 Material
We used single crystals with hexagonal/square shape with a diameter between 80 and 140 tam. as well as polycrystalline material (particle size of ~ 1 tam). Both samples were provided by Dr. H. Kessler, Laboratoire de Mat6riaux Min6raux, Ecole Nationale Sup6rieure de Chimie, Mulhouse. Cloverite possesses two non intersecting 3-dimensional pore systems. The large pore system consists 20 membered rings with a free diameter of approximately 1.3 nm, the other pore
72 system is formed by 8 membered rings showing a free diameter of only -0.4 nm. At the intersections of the large pores, supercages are formed which exhibit a diagonal diameter of 2.9 nm [1-3]. The lattice of cloverite is neutral consisting of alternating PO4- and GaO4- tetrahedra. The terminal hydroxyl groups which are an integral part of the lattice are located in the large pore system (see fig. 1).
absorbanee [ar units] __
3702 C-aOH
3675 POH
.
.
-
.
.
..-.
" ;"'"
I 0 . 8
--
~~
0.6 0.4
. "',G a O H
POH .
I
i
.o.5! m .
0.2 0 3800
1
3300
I
2800
I
I
I
2300
1800
1300
wavenumbar [1/em]
Figure 1" Spectrum of the activated cloverite and graphic representation of a part of the unit cell (enlarged, the part where the structural hydroxyl groups are situated). In the representation of the part of the unit cell, only the T-atoms are connected
2.2 Sorption studies Activation, sorption and desorption were followed in situ by time resolved FTIR microscopy. The measurements on the single crystals were carried out in a vacuum cell equipped with i.r. transparent windows attached to the stage of a BRUKER i.r. microscope. The spectrometer used was a BRUKER IFS 88 (4 cmq spectral resolution). The polycrystalline material was pressed into self supporting wafers and measured in another high vacuum cell which was placed in the BRUKER IFS 88 spectrometer. This cell was connected to a B ALZERS QMG 410 mass spectrometer which was used to monitor the gas phase composition during temperature programmed desorption. The template was removed by heating the sample with 10 K/min up to 800 K in air, holding this temperature for two hours and subsequently evacuating the system to 10-6 mbar and cooling it to 300 K to perform the sorption experiments. The structure of the activated molecular sieve was stable in vacuum or inert gas atmosphere. The sorbates were introduced into the reaction cell via a gas inlet system at a temperature of 300 K. The desired partial pressure was held constant until sorption/desorption equilibrium was achieved and was then increased in steps from 10.3 to
73 1 mbar. Subsequently, the system was again evacuated to 106 mbar for 90 minutes, followed by temperature programmed desorption (TPD, heating rate 10 K/min, final temperature between 800 and 900 K). 3. RESULTS AND DISCUSSION 3.1 Acid sites in cloverite The i.r. spectrum of the activated cloverite (fig. 1) showed two absorption bands at 3702 and 3675 cm~, which are assigned to Ga-OH and P-OH groups, respectively [8]. Upon sorption of benzene, the i.r. bands of these OH groups were broadened and shifted to lower wavenumbers (A v = 250 crn~ for the Ga-OH and 220 cm~ for the P-OH group, compared to the 260 cm~ shift observed for SiOHAI groups of HZSM-5). Because the magnitude of the red shift of the OH bands after adsorption of a donor molecule is directly proportional to the acid strength of the OH group [9], this indicates high and moderate acid strength of the OH groups of cloverite. The absorption bands in the spectral region below 2500 cmx are assigned to overtones and combinations of the lattice vibrations of the gallium phosphate [ 10]. 3.2 Sorption of strong bases The nature and accessibility of the acid sites in cloverite was probed by sorption of three bases molecules, ammonia, pyridine and trimethylamine (TMA). These molecules have different proton affinities and kinetic diameters, with ammonia having the lowest proton affinity and the smallest kinetic diameter. The i.r. spectra of ammonia and pyridine sorbed on cloverite show characteristic absorption bands for Lewis (1616 c m "1 for ammonia and 1613 cm~ for pyridine) as well as Bronsted (1450 cm1 for ammonia and 1543 cm1 for pyridine) bonded species [11]. With increasing coverage, the absorption bands of both species increased parallel in intensity, while the intensity of both types of OH groups decreased. It should be emphasized that preferential sorption on one of the sorption sites (Ga-OH or P-OH groups) was not found. After equilibration at 0.1 mbar at 300 K, all hydroxyl groups were found to interact with base molecules. Bonding to cloverite was concluded to be strong, as desorption did not occur upon evacuation at 300 K. During temperature programmed desorption (TPD), pyridine and TMA desorbed first from the P-OH group (maxima of the rate of desorption around 800 K). The molecules interacting with the Ga-OH groups could only be partially desorbed up to 900 K in vacuum, but were completely removed upon treatment in flowing air at 800 K. This unusual high thermal stability and the simultaneous disappearance of the free hydroxyl groups and the appearance of the bands characteristic for Lewis and Br6nsted bonded species led us to conclude that the Bronsted acidity of cloverite cannot account alone for the strong sorption of the base molecules. For ammonia, the removal of the molecules by the above described thermal treatments (900 K in vacuum, 800 K in air) did not lead to the reappearance of the OH stretching vibration bands characteristic for the cloverite structure. Then, only a small band at 3675 cm~ characteristic for P-OH groups was observed. This spectrum was similar to that recorded after sorption of water at ambient temperature (followed by TPD) which led to a collapse of the microporous structure [2]. In agreement with Patarin et a/.[3] we therefore conclude that the same occurs in the presence of ammonia at elevated temperatures. An amorphization of cloverite after a stepwise thermal desorption of ammonia was confirmed by XRD measurements [3].
74 As pyridine and TMA have stronger gas phase basicities than ammonia and their sorption did not lead to an irreversible change/damage of the lattice, we conclude the size of the molecule to be a decisive factor for the destabilization of the cloverite structure. These results clearly indicate that a concerted interaction of Br6nsted and Lewis acid sites occurs upon sorption of the base molecules on cloverite. This concept of a concerted interaction of Lewis and Br6nsted acid sites implies that upon sorption, one of the Ga-O bonds next to the Ga-OH group is partially opened and that the primary interaction takes place between the then accessible Ga cation and the base molecule. This might induce a rehybridization of the Ga cation from tetrahedral symmetry first to a 5-fold coordination (like it is present in the "as synthesized" form) and then to complete octahedral (corresponding to 6fold) coordination (fig.2). The 6-fold coordination is possible for the smaller ammonia molecules, as they can enter also the small pore system (free inner diameter -0.4 nm) and coordinate to the Ga cations through the double 4 tings connecting the large with the small pore system (as shown in figs. 1 and 2). For the larger pyridine and TMA molecules a cleavage of the Ga-O bond still occurs and leads to a Lewis type coordination between the Ga cation and the base molecule. However, the additional interaction of a second molecule via the small pore system cannot be achieved leading only to a five fold coordination of the Ga upon sorption of these molecules.
Ga in 4ofold coordination (activated sample)
Ga{
Ga in 5-fold coordination
ammonia
G a in 6-fold coordination
ammonia
ammonia
Figure 2: Change in coordination of gallium upon sorption of ammonia
75
3.2 Sorption of alcohols While the sorption of the strongly basic molecules occurred in parallel on both types of hydroxyl groups, preferential interaction with the Ga-OH groups was noticed with the alcohols (methanol, ethanol and propanol). This effect was quite pronounced with methanol and decreased in importance with increasing molecular weight of the alcohol. Note that all Ga-OH groups interacted with an alcohol molecule at rather low partial pressures (10 .3 mbar), while the partial pressures required to cover all P-OH groups were decreased with increasing chain length (see table 1). Tablel Uptake characteristics of alcohols on Br6nsted acid sites Alcohol
O0,.on) at O(Ga.ori)= 1 [1]
Peq. to reach Oo,.ori)=1 [mbar]
Methanol
0
1
Ethanol
0.25
0.1
Propanol
0.6
0.01
O ...... coverage Peq.. ..... equilibrium pressure After equilibration with 10s mbar, all Ga-OH groups interacted with methanol molecules. The i.r. spectra of the sorbed species recorded during the uptake of methanol suggest the existence of two different sorption structures on the Ga-OH groups [8]. At low coverages, structure A which is characterized by bands of the CH stretching vibrations at 2828 and 2940 cm1, was dominant. After longer exposure (corresponds also to higher coverages) a shoulder rose at 2838 cm1 and a new peak appeared at 2950 cm~ . These bands were attributed to a second sorption structure of methanol (structure B). Under these conditions, the P-OH groups were not affected by methanol adsorption. At partial pressures higher than 10.3 mbar, methanol interacted also with the P-OH groups causing bands of CH stretching vibrations at 3000, 2962 and 2855 cm~ (structure C). These absorption maxima are close to those observed for methanol hydrogen bonded to weakly acidic silanol groups (3001, 2958 and 2856 cm1) [12]. Thus, we suggest a similar type of interaction for methanol sorbed on the P-OH groups of cloverite. It should be emphasized that the bands of the CH stretching vibrations of methanol interacting with the Ga-OH groups occurred at quite low wavenumbers, comparable only with the values observed for methanol sorbed on Rb- of Cs-cations in alkali exchanged X-zeolites [ 13]. This led us to conclude that the interaction of methanol with the Ga-OH groups cannot be ascribed to hydrogen bonding or protonation like in other acidic zeolites [ 14], but an additional interaction of the hydrogen bonded molecules with Lewis type sites has to be assumed. Based on these results and the evidences collected for the sorption of strong bases, we conclude that also upon sorption of methanol, a Ga-O bond neighboring the Ga-OH group is broken creating a strong Lewis acid site next to the hydroxyl group.
76 The i.r. spectra of ethanol and propanol sorbed on cloverite showed only absorption features characteristic for an alcohol molecule interacting via hydrogen bonds with acidic hydroxyl groups [ 14]. Thus, it is difficult to judge whether ethanol and propanol are polar enough to cause the same type of lattice opening as it was observed with methanol. Upon evacuating the system, almost complete desorption of methanol and ethanol from the P-OH groups was observed. However, about 30 ~ of the P-OH groups still showed interaction with propanol under these conditions. Such a behavior can only be explained, if we assume that propanol interacts with the P-OH and the Ga-OH groups simultaneously. This seems possible because of the steric vicinity of the two structural OH groups (average distance absorbaace [ark units] between them is 0,51 nm and the length I 28~g of the propanol molecule is 0,53 rim. See / ~ 2835~' also fig.1.). It should be noted that 0.15 J~% evacuation at ambient temperature did not affect the interaction of the alcohol molecules with the Ga-OH groups. 300 K In addition to unreacted methanol, "/;'|~ Y / / / ~ ~ . . ~ ~ / ~ ~ ~ ~ the formation of two different products, [~/. dimethylether and formaldehyde was observed during temperature ~ ~ ~ ~ ~ programmed desorption ( T P D ) o f methanol from cloverite. The i.r.spectra 1 ~ ~ recorded during TPD of methanol from 0 900 K polycrystalline cloverite are shown in fig.3. Dimethylether formation occurred 3000 ~ ~ ~ 2800 r at lower temperatures (maximum rate of waveaumber [l/m] desorption around 500 K) and is directly correlated to the disappearance of structure B from the surface. The other sorption species (mainly species A) Figure 3: I.r. spectra recorded during TPD of desorbed as formaldehyde at higher methanol from cloverite temperatures (maximum rate of desorption around 670 K). Upon increasing the temperature, ethanol and propanol desorbed partly unreacted from the Ga-OH groups. At temperatures above 500 K, dehydration of the alcohols took place leading to the formation of water, ethene and propene. Other reaction products were not detected by mass spectrometry. 4. CONCLUSIONS The structural hydroxyl groups of cloverite exhibit high and moderate Bronsted acid strength towards apolar hydrocarbon molecules. With polar molecules, these hydroxyl groups show unique interactions leading to a local rearrangement of the lattice including a breaking of the Ga-O bond close to the Ga-OH sorption site. Consequently, a concerted Lewis and Br6nsted acid type interaction is concluded to exist between the basic molecules and the Ga-OH/Ga cation sorption
77 sites. This type of interaction is paralleled by a change in the coordination of the Ga cation to first 5-fold (upon sorption of 1 probe molecule) and then, after sorption of a second molecule to complete 6-fold (octahedral) coordination. This 6-fold coordination can only be achieved, if the probe molecule is small enough (like water or ammonia) to enter the small pore system and to coordinate to the Ga cation via the double 4 tings. Desorption of the molecules from the octahedral coordination, leads to a collapse of the microporous structure of cloverite and results in the formation of an amorphous G a P O 4. Methanol sorbs preferentially on the Ga-OH groups leading to two different sorption structures. One coordinatively bound species to Ga cations which desorbs reactively as formaldehyde at elevated temperatures. The other structure is attributed to methanol hydrogen bonded to the Ga-OH groups and yields dimethylether upon desorption. ACKNOWLEDGEMENT
The work was partially founded by the Christian Doppler Laboratory for Heterogeneous Catalysis. The graphic displays shown in figures 1 and 2 were printed out from the I N S I G H T H molecular modeling system (BIOSYM Technologies Inc.). We thank Dr.Henri Kessler for providing the cloverite samples. REFERENCES
.
.
.
7. 8.
9. 10. 11. 12. 13. 14.
M.Esterman, L.B.McCusker, C.Baerlocher, A.Merrouche and H.Kessler, Nature 352 (1991)320. A.Merrouche, J.Patarin, H.Kessler, M.Soulard, L.Delmotte, J.L.Guth and J.F.Joly, Zeolites 12 (1992) 226. J.Patarin, C.Schott, A.Merrouche, H.Kessler, M.Soulard, L.Delmotte, J.L.Guth and J.F.Joly, Proc. 9th IZC; van Ballmoos, R. et al.; Butterworth-Heinemann, 1993, 263. R.L.Bedard, C.L.Bowes, N.Combes, A.J.Holmes, T.Jiang, S.J.Kirkby, P.M.Macdonald, A.M.Malek, G.A.Ozin, S.Petrov, N.Plavac, R.A.Ramik, M.R.Steele, and D.J.Young, Am. Chem. Soc. 115 (1993) 2300. B.Zibrowius, M.W.Anderson, W.Schmidt, F.F.Scht~th, A.E.Aliev and K.D.Harris, Zeolites 1993, 13,607. T.L.Barr, J.Klinowski, H.He, K.Alberti, G.Mtiller and J.A.Lercher, Nature 365 (1993) 429. S.Bradley, R.F.Howe and J.V.Hanna, Solid State Nuclear Magn. Res. 2 (1993) 37. G.Mt~ller, G.Eder-Mirth, H.Kessler and J.A.Lercher, J.Phys.Chem. submitted 1995. M.L.Hair and W.Hertl, J. Phys. Chem. 74 (1970) 91. V.V.Krymova, L.E.Kitaev, A.A.Kubasov, Z.V.Gryaznova, L.S.Eshchenko and V.V. Pechkovskii, Vestn. Mosk. Univ., Ser. 2. Khim. 20(5) (1979) 476. L.H.Little, "Infrared Spectra of Adsorbed Species", Academic Press, London, 1966. E.P.Parry, J. Catal. 2 (1963) 371. B.A.Morrow, J.Chem.Soc.Farad.I 70 (1974) 1527. G.Eder-Mirth, H.Wanzenb6ck and J.A.Lercher, ZEOCAT 95, accepted for publication. M.T.Aronson, R.J.Gorte and W.E.Farneth, J.Catal. 105 (1987) 455. G.Mirth, A.Kogelbauer and J.A.Lercher, Proc. 9th IZC; van Ballmoos, R. et al.; Butterworth-Heinemann, 1993, 251.
This page intentionally left blank
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
79
Brgfnsted sites of enhanced acidity in zeolites: experimental modelling M.A.Makarova*, S.P.Bates** and J.Dwyer Chemistry Department, UMIST, PO Box 88, Manchester M60 1QD, UK
Low-temperature interaction of BF3 with acid forms of zeolites is shown to take place in two different ways: as an amphoteric complex (I) and as an acid-base complex (11). These complexes are observed using FTIR spectroscopy and their assignment is based on theoretical calculations. In the case of BF3/H-ZSM-5 only the weaker bonded complex (11) is observed, whereas in the BF3/H-EMT system both types of complexes are present. Formation of amphoteric complex (I) affects the acid strength of the remaining uncomplexed Brensted hydroxyls (as shown by lowtemperature adsorption of CO on the samples pretreated with BF3). This provides for the first time experimental proof that enhanced Bronsted acidity may result from interaction of acid forms of zeolites with Lewis acids. In contrast, formation of complex (11)does not affect the acidity of the zeolite. The fact that formation of complex (I) was not observed in the case of the BF3/H-ZSM-5 system indicates the significance of AI content and/or topological factors for creation of enhanced acidity in zeolites.
1. INTRODUCTION The nature of enhanced Brensted acidity remains one of the key questions in mechanistic studies of the acid-base reactions on zeolites. The enhancement in acid strength is believed to be a result of the interaction between Bronsted sites and Lewis sites created during steaming procedures, since both are present, and since it is known that, in solution, enhanced Brensted acidity can be generated by adding Lewis acid to Bronsted acid [1]. However, as yet there is no direct proof that Lewis sites participate in the enhancement of Brensted acidity. The present study deals with reversible adsorption of a Lewis acid, BF3, on two zeolite materials in the H-form: EMT and ZSM-5, with the aim of creating a model system which demonstrates enhanced acidity without destruction of the zeolitic framework.
* Present address: Koninklijke/Shell Laboratorium, Amsterdam, Postbus 38000, 1003 BN Amsterdam, The Netherlands ** Present address: Laboratory for Inorganic Chemistry and Catalysis, Eindhoven University of Technology, P.O.Box 513, 5600 MB Eindhoven, The Netherlands
80 2, E X P E R I M E N T A L
Carbon monoxide was supplied by BOC (R grade) and boron trifluoride by Aldrich (99.95%+). Two zeolite samples, H-EMT (Si/AI = 4, Na/AI < 0.01) and HZSM-5 (Si/AI = 16, Na/AI < 0.01) were used. 29Si MAS NMR and 27AI MAS NMR proved the absence of dislodged aluminium. The FTIR spectroscopic technique was described in detail elsewhere [2]. Briefly, an infrared cell facilitated high temperature pretreatment of the samples in-situ, and was on-line with the adsorption rig. A self-supporting disk (m - 5-10 mg, p ~ 5 mg. cm 2) was heated at l~ 1 to 350~ under vacuum and held at this temperature overnight (pressure of 10STorr). For spectroscopic/adsorption measurements, the IR cell was lowered into a quartz Dewar filled with liquid nitrogen and small doses of BF3 or CO (0.4 - 1.0/~mol) were admitted to the cell. Adjustment of the sample position within the cell permitted placement of the sample in regions of different temperature. Thus, the temperature of the sample during adsorption/desorption of BF3 ranged from -40 to -100~ during CO adsorption and spectra registration it ranged from -100 to -120~ The spectra were collected using a Cygnus-100 Mattson FTIR spectrometer, at a scanning rate of 100 and a resolution of 2cm 1 in the wavenumoer interval of 2500 4000cm ~ . A single-beam spectrum of thecell (including the quartz Dewar and liquid nitrogen) was used as background. The shifts, ~vOH, due to perturbation with carbon monoxide were determined as peak-to-peak distances in difference spectra obtained by subtraction of the spectra of the samples before adsorption from their spectra after adsorption.
3. RESULTS 3.1 BF 3 interaction with H - E M T
FTIR spectra of the initial H-EMT material and that after low-temperature adsorption of BF3 are shown in Fig. 1. As a result of interaction, the intensity of the high frequency band decreases and new broader bands at 3267cm 1 and 3472cm 1 appear. These new bands most probably correspond to stretching vibrations of Bronsted hydroxyls involved in hydrogen-bonded interaction with adsorbed BF 3 molecules. The adsorption is completely reversible and prolonged pumping at room temperature restores the spectrum of the initial sample. The band at 3472cm 1 disappears after low-temperature evacuation, while the band at 3267cmJ is unchanged. This indicates that the two observed spectroscopic bands can be assigned to different types of adsorption complexes: a stronger complex (I) characterised by the OH stretching vibration at 3267 cm 1 and the weaker complex (It) corresponding to the band at 3472cm ~ . Formation of complex (I) affects the acid strength of the remaining hydroxyls. This conclusion is reached from the results of low temperature adsorption studies of carbon monoxide. The method is based on measurements of the shift in the position of the hydroxyls, AVON, due to their perturbation with CO (at =-120~ [3-5]. Briefly, the larger the shift, the more acidic the hydroxyls. The proton affinities of the hydroxyls and their shifts are related by: PATM / kJ.mol 1 = 2254.8- 442.5 log
(AVOH/
cm 1 )
81
b
,
~__~
S
i
b
/ C
e
1
38'00
'
3400 Naven
1
1
3000
I
1
2600
mbens
Figure 1. FTIR spectra of H-EMT on exposure to BF3: a) initial sample, b) after low temperature adsorption of excess BF3, c) after subsequent low-temperature evacuation.
The shift determined at the limit 0co-,0 (low coverage) reflects the acid strength of the strongest hydroxyls whereas the extrapolation to eco-,1 (high coverage) corresponds to their average acidity. In the present experiment, the fractional coverages with the sorbates were determined from the spectroscopic results as follows: 0BF3 is the decrease in I(HF) (intensity of the high frequency band) due to BF3 adsorption divided by I(HF) before any adsorption; - 0co is the decrease in I(HF) due to BF3 and CO adsorption divided by I(HF) after BF3 adsorption only; - 0 B F 3 + c o i S the decrease in I(HF) due to BF3 and CO adsorption divided by I(HF) before any adsorption. Consequently, Oco = (eBF3+CO- OBF3)/(1 - OBF3). -
82
400 Mathematical treatment of the experimental results on CO adsorption in terms of plots of A v OH VS. OBF3+COfor different starting 0BF3 is given in Fig.2. The different lines correspond to different starting 0BF3 and the crosses at the end of each line correspond to their values in the series of adsorptions of CO. The shifts due to CO perturbation, A YON, become larger as more BF3 is preadsorbed in the form of complex (I). This is direct evidence of the enhancement of the strength of Bronsted hydroxyls resulting from the interaction of the zeolite with BF3 without destruction of the zeolitic lattice. In general, it proves, for the first time the hypothesis that enhanced Brensted acidity can be formed by the interaction of Brensted sites with Lewis acids or Lewis acid sites.
380
360 T
o ~
3/+0
<1 320
300 a
280
260
0
0;2
016 0;8 0BF 3 + CO
Figure 2. Shift in the position of the HF hydroxylsdue to perturbation with carbon monoxide vs. the fractional coverages of the HF hydroxyls with both sorbates, BF3 and CO.
3.2 BF 3 interaction with H - Z S M - 5
FIIR spectra corresponding to low-temperature adsorption of BF3 on H-ZSM-5 are shown in Fig.3. Only one band at 3494cm 1 arises as a result of interaction, accompanied by the decrease in the hydroxyl band from Brensted hydroxyls at 3619cm 1. Therefore, low temperature adsorption of BF3 on H-ZSM-5 results in preferential formation of complex (11). Experiments on carbon monoxide adsorption for acidity measurements, similar to those described above, show no increase in the acid strength of the Bronsted hydroxyls as a result of formation of complex (11). The shift in their position after perturbation with CO, AVON, stays approximately the same, ~310cm 1 , independently on the amount of BF3 preadsorbed, and corresponds to the shift, observed previously for the unmodified H-ZSM-5 sample [5].
4. D I S C U S S I O N
Ab initio HF/SCF molecular orbital calculations (using the 3-21G basis set in
GAUSSIAN92 [6]) show that the most stable adsorption complex is based on an 8-ring cycle and involves zeolite - BF 3 amphoteric interaction :
83 This structure is assigned, Broensted therefore, to the spectroscopically ~O F t", " , acid - base observed complex (I). The predicted .~.H. \ ""r- I complex is characterised by a two-point i . .r-~_.. interaction: a strong H-bond between & I ' B L . _ ~ Lewis BF3 and the Brensted hydrogen and a strong B-O bond, 0.2 ~ longer than the bond lengths observed in boron trioxide and B(OH)3 [7]. No stable complex exists when the B atom interacts with the framework oxygen immediately adjacent to the aluminium atom (in contrast to calculations involving other bases that are predicted to coordinate via two points, such as methanol and ammonia [8, 9]). A complex of this type is not stable for this system due to repulsion effects between the framework and the out-of-plane F atoms.
/I
i b 0.2
S 0 p
b a r]
_ _ _
C e
'
sBbo
1 .....
s4bo
I
sobo
~Aavenumbens Figure 3. FTIR spectra of H-ZSM-5 on exposure to BF3. a) initial sample, b) after low temperature adsorption of excess BF3.
I
26bo
84 The HF interaction energy of the complex shown above is 238 kJ/mol. The small basis set used for these calculations is subject to a considerable Basis Set Superposition Error (BSSE) [10]. This artificially increases the interaction energy by 102 kJ/mol, according to the method detailed in Ref.11. The effects of electron correlation are included via single point Moller-Plesset calculations (MP2) at the SCF optimised geometries. This correction decreases the interaction energy by 5 kJ/mol. (This destabUisation is in contrast to previous MP2 calculations which stabilise the complexes of CO and methanol on a Bronsted acid-site model [8, 11]). The framework oxygen acting as a Lewis base to BF3 is within 4~ of sp 2 hybridisation, thus maximising electron donation. The hybridisation at this oxygen is likely to be intermediate between sp (180~ and sp 2 (120 ~ in the real zeolite, thus reducing the efficiency of electron donation. To estimate the size of this, calculations have been performed with this SiOH angle fixed at 150~ A reduction in SCF interaction energy of 20% is observed. Thus the final estimate of the interaction energy is 102 kJ/mol. The spectroscopic pattern for Bronsted hydroxyls interacting to give complex (11), is typical for hydrogen-bonding perturbation by weak bases such as CH 4 - C6H14 [12] or CHF 3 [13]. Thus the following structure can be proposed for complex (11): m
zAI / O - H...F3B si
"
In this pair BF3 behaves only as a weak base interacting with an acid, which in this case is the zeolite Bronsted hydroxyl. Enhancement of the acidity of the remaining, uncomplexed Bronsted hydroxyls in the case of formation of complex (I) on one hand, and the absence of any effect in the case of formation of complex (11), on the other, concurs with our assignments. A possible mechanism for enhancement of acidity could involve electron density withdrawal from appropriate zeolite oxygen atoms. The fact that complex (I) can be easily formed during BF3 adsorption on H-EMT but not on H-ZSM-5, may have the following reasons. Firstly, the space inside the 10rings of ZSM-5 channels may be insufficient for proper orientation of the BF3 molecule for the 2-point interaction necessary for complex (I). This is illustrated in Fig.4: BF3 has much more space and freedom in the 12-ring of EMT channels for the formation of the complex of preferred geometry. Secondly, it may arise from the different Si/AI ratio in the two zeolites used, which can result in different acidity of the hydroxyls and different bacisity of the framework oxygens, thus changing the affinity of the zeolite towards formation of complex (I). Finally, it is important to note, that behaviour of these two zeolite materials in terms of enhancement of Bronsted acidity due to interaction with Lewis acid BF3 is in remarkable parallel with enhancement of their acidity as a result of steaming. The increase of catalytic activity is much more prominent in the case of US-Y catalysts (steamed faujesite, structure similar to EMT)[14] as compared to steamed H-ZSM-5
[15].
85
Figure 4. Visualisation of a BF3 molecule adsorbed in the zeolite channels of a) ZSM-5; b) EMT
86 ACKNOWLEDGEMENTS
We thank Drs. P.Schultz and T.Des Courieres (Elf France) for H-EMT sample preparation; Prof. V.B.Kazansky (Zelinsky Institute of Organic Chemistry), Dr. A.M.Rigby (Shell Research), Drs. J.Dewing, V.Zholobenko and C.Cundy (UMIST) for useful ideas and discussions. We are also grateful to the EC (BRITE EURAM 4633) for financial support for M.A.M.
REFERENCES .
2. .
4 . .
5. .
.
.
9 10 11 12 13. 14. 15.
C. Mirodatos and D. Barthomeuf, J.Chem.Soc.Chem.Commun., (1981), 39. M.A. Makarova, V.L. Zholobenko, K.M. AI-Ghefaili, N.E. Thompson, J. Dewing and J. Dwyer, J.Chem.Soc.Farad.Trans., 90 (1994) 1047. E.A. Paukshtis and E.N. Yurchenko, Usp.Khim., 53 (1983) 426. L. Kubelkova, S. Beran and J.A. Lercher, Zeolites, 9 (1989) 539. M.A. Makarova, K.M. AI-Ghefaili and J. Dwyer, J.Chem.Soc.Farad.Trans., 90 (1994) 383. M.J. Frisch, G.W. Trucks, M. Head-Gordon, P.M.W. Gill, M.W. Wong, J.B. Foresman, B.G. Johnson, H.B. Schlegel, M.A. Robb, E.S. Replogle, R. Gomperts, J.L. Andres, K. Raghavachari, J.S. Binkley, C. Gonzalez, R.L. Martin, D.J. Fox, D.J. Defrees, J. Baker, J.J.P. Stewart, J.A. Pople, Gaussian 92, Rev. E.1; Gaussian Inc., Pittsburgh PA, 1992. A.F. Wells, Structural Inorganic Chemistry, 5th Ed., Clarendon Press, Oxford, 1984. S.P. Bates and J. Dwyer, J. Mol. Struct. (THEOCHEM), 306 (1994) 57. E.H. Teunissen, R.A. van Santen, A.P.J. Jansen and F.B. van Duijneveldt, J.Phys. Chem., 97 (1993) 203. J. Sauer, Chem. Rev., 89 (1989) 199. S.P. Bates and J. Dwyer, J. Phys. Chem., 97 (1993) 5897. M.A. Makarova, A.F. Ojo, K. Karim, M. Hunger and J. Dwyer, J.Phys.Chem., 98 (1994) 3619. M.A. Makarova, unpublished results. F. Lonyi and J.H. Lunsford, J.Catal., 136 (1992) 566. R.M. Lago, W.O. Haag, R.J. Mikovsky, D.H. Olson, S.D. Hellring, K.D. Schmitt and G.T. Kerr, Stud.Surf.Sci.Catal., 28 (1986) 677.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviotand S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
87
M o d e l l i n g of s t r u c t u r e a n d r e a c t i v i t y in zeolites C.R.A. Catlow a, R.G. Bell a, J.D. Gale b and D.W. Lewis a aThe Royal Institution of Great Britain, 21 Albemarle Street, London WIX 4BS UK bDepartment of Chemistry, Imperial College of Science, Technology and Medicine, Exhibition Road, London SW7 2AZ 1.
INTRODUCTION Computer modelling techniques are now well established as powerful tools in the study of microporous solids [1-3]. In this article we highlight recent applications using both forcefield and electronic structure techniques to the study of problems in structure, sorption, synthesis and reactivity of both zeolites and microporous aluminophosphates. In particular, we describe how simulation techniques can yield detailed and accurate information of the structure and energies associated with framework modification by hetero-atoms; on the diffusion coefficients and migration mechanisms of sorbed molecules; on the nature of the interactions between host structures and templates used in zeolite synthesis; and on the use of electronic structure techniques in throwing light on the crucial questions of acid site-molecule interactions in solid acid catalysts. In the next section we summarise the range and status of the current computational methodologies before describing the recent illustrative applications. We conclude with consideration of the likely future direction for the field. 2.
METHODOLOGIES The full range of contemporary computer simulation techniques are available for the simulation of microporous systems, and detailed accounts are available in, for example, reference [1]. The present section concentrates on recent developments.
Forcefield methods (i.e. techniques which rest on the specification of interatomic potentials) have been used extensively in modelling the structures of microporous solids and in investigating docking and diffusion of sorbed molecules [1]. The full range of simulation techniques m Energy Minimisation (EM), Monte Carlo (MC) and Molecular Dynamics (MD) have been employed, as have combinations of these methods, as in the widely used 'docking' procedure developed by Freeman and coworkers [4] for identifying low energy sites for sorbed molecules. It is a truism that the reliability of such simulation depends
88 upon the quality of the interatomic potential models employed. Two types of model are used in current studies: first Born model potentials with a shell model treatment of polarisability, which considers the solid in terms of ions interacting via long-range (Coulombic) and short-range potentials. Models based on both formal [5] and partial charges [6-7] are available. Both perform well in modelling structures of zeolites [8] although interestingly, a recent careful evaluation of energy minimised compared to high quality crystallographic data [9] suggested that the earlier formal charge model of Sanders et al. [5] generates the most accurate structures. An alternative approach is provided by "molecular mechanics" forcefields which treat the solid in terms of a covalently bonded network with energy terms depending on the extent of stretching, bending and rotation of bonds from equilibrium values. Again, a number of such parameter sets are available for zeolites [10-11] which work well in modelling structures. Parameters may be derived for both types of forcefield using either empirical methods in which the parameters are adjusted via a least square fitting procedure in order to reproduce the structure and properties of model compounds as closely as possible. Recent work has, however, placed increasing emphasis on the use of ab initio electronic structure techniques to calculate the energy of a periodic array or cluster of atoms, whose geometry is then varied in a systematic manner with the resulting energy surface being fitted to the interatomic potential function. Examples of such an approach are the parameter sets derived by van Beest et al. [6], Purton et al. [7] and Hill and Sauer [11]. As noted, both Born and molecular mechanics models have enjoyed success in modelling zeolites [8-12] as might indeed be expected in view of the character of the Si-O bond which is intermediate between ionic and covalent. In general, Born model potentials are more flexible and allow the inclusion of cations in a more f r a m e w o r k h e t e r o - a t o m s and e x t r a - f r a m e w o r k straightforward manner. Molecular mechanics potentials may possibly represent more accurately the response of the framework to sorbed molecules. Parameters for molecule-framework interaction still rest largely on empirical studies of sorption enthalpies, as in the widely used set for hydrocarbons due to Kiselev [13], while for more complex molecules e.g. alcohols and amines, parameters are generally 'borrowed' from sets developed for organic/biological systems. And, although several successful studies have been reported employing such parameters, there is a clear requirement for more reliably based parameter sets derived from ab initio calculations. The need for such parameterisation will grow as studies extend to an increasingly wide range of microporous solids containing a greater variety of atom types. The most important recent technical developments in the field of simulation concern first the growing use of Grand Canonical Monte Carlo (GCMC) methods to simulate sorption isotherms (as in the recent work of Gorman et al. [14], and increasingly sophisticated 'docking' procedures for locating molecules, especially template species, within zeolite pores; further discussion of the latter will follow below. A further significant development concerns molecular dynamics techniques, which have been used extensively in modelling molecules in zeolites for a period of more than ten years; such
89 techniques are beginning to find a wider range of applications owing to the availability of massively parallel processors which are ideal for undertaking long time scale simulations of the diffusion of sorbed molecules. Such calculations are needed for reliable simulation studies of diffusivity in microporous solids. Overall, simulation studies using interatomic potentials are now a standard technique in zeolite science, with the trend in current work being towards the refinement of interatomic potential parameters and their extension to new types of interactions, and with continuing development and adaptation of simulation techniques to new computer architectures and new problems. The use of explicit electronic structure techniques has also grown considerably during recent years. As noted, such techniques are of importance in the derivation of high quality interatomic potentials. But of even greater significance is their increasing use in modelling fundamental features relating to reactivity including acid site-molecule interactions [2], [15-19] and reaction mechanisms of molecules sorbed at both Br~nsted acid centres [2] and extraframework transition metal ions. The full range of current semi-empirical and ab initio techniques have been employed in electronic structure studies of zeolites, and reviews of both approaches are given by Vetrivel in reference [1] and by Sauer and coworkers in references [1] and [3]. Semi-empirical techniques, if well parameterised, may prove effective in modelling structures and stabilities. Recent work has, however, emphasised the use of ab initio techniques, which, due to algorithmic and hardware developments, may be applied to increasingly large and complex systems. Calculations may be performed on clusters of atoms (as in the majority of studies of zeolitic systems) or on periodic arrays, as in the recent ab initio Hartree Fock studies of Hess and coworkers [20]. Other important features of recent work have concerned the use of large clusters as in the work of Sauer et al. [3], [11], [17]; the location of transition states for reaction mechanisms [2], [16]; and the use of Local Density Functional (LDF) in addition to Hartree Fock (HF) methodologies [16]. The value of the use of the latter techniques on large scale clusters will be evident from the recent work on acid site-methanol interactions described later in this paper. 3.
APPLICATIONS To illustrate the present range and status of computational techniques in zeolite science, we have chosen to highlight recent applications concerning problems in structure, sorption and diffusion, templating and molecule-acid site interactions - - examples which reveal both the strengths and limitations of current approaches. 3.1.
Structural studies of framework hetero atoms in zeolites Manipulation of microporous materials by inclusion of framework substituting metal atoms is an increasingly common method of modifying their properties (including catalytic behaviour). Simulations are an effective tool for studying the structures of such materials and are particularly useful when
90 applied together with experimental techniques such as EXAFS, as the two following recent examples show. 3.1.1. Structural properties of Fe/ZSM-5 Fe modified ZSM-5 has been widely investigated because of the modification effected to its catalytic properties[21]. Although it has been well established that the material can be prepared with predominantly framework substituted Fe, the determination of the detailed structure of the localised state created on substituting Si by Fe is not straightforward. The topic is, however, an ideal one for investigation by contemporary computer modelling techniques. As good interatomic potentials are available for interactions involving all the relevant species, we can generate accurate models for the substitutional site. The most stable structures involve protonation of the neighbouring oxygen site to give the structure shown in Figure 1, in which the Fe atoms form three shorter Fe...O bonds and one longer one to the protonated site. Lewis et al. [22] were able to show that this structure accords very well with earlier EXAFS data of Axon et al. [23]. Indeed, they found that the observed spectra were within experimental error of those calculated from the simulated structures. In addition, the simulations were able to give improved models for the location of the template in the pores of the zeolite with respect to the Fe substitutional. Moreover, they showed how the iron substitutional causes interesting and subtle distortion of the pore geometries which are almost certainly responsible for modifications in the relative diffusivity of sorbed molecules which in turn effect the observed changes in the shape selectivity of these catalysts. 3.1.2. Titanium environments in titanosilicates There is an increasing interest in titanium-containing microporous and mesoporous silicates, due to their catalytic performance for the oxidation of organic compounds under mild conditions as well as their ion-exchange properties [24-30]. In most of these materials, the titanium is located at tetrahedral framework sites [31-34]; however a recently-synthesised class of titanosilicates [35-37], including ETS-10, exists in which Ti 4+ is octahedrally coordinated.
The basic structure of ETS-10 was recently elucidated by Anderson and coworkers [38-40], employing a combination of 29Si NMR, electron microscopy and power X-ray diffraction (using distance-least-squares refinement of bond lengths and angles). The framework is characterised by possessing 12-ring channels running in two orthogonal directions, and also by two sets of Ti-O-Ti chains which run parallel to these channels. Each titanium atom enjoys six-fold coordination, having four Ti-O-Si linkages in addition to the two Ti-O bonds along the chain direction. It was not possible however to obtain a detailed description of the structure by these experimental means, since ETS-10 exists as a highly disordered intergrowth of two polymorphs which differ in the stacking sequence of the 12-ring pores, and also because only powder samples with small particle sizes could be obtained. The structural models assumed a high degree of crystal symmetry which, for instance, constrained all Ti-O bonds to be between 1.87 and 1.91A in length, and moreover were unable to take into account the
91 extra-framework alkali metals ions which are necessary to maintain the charge neutrality of the structure. A further refinement of the local structure around titanium was achieved using a combination of x-ray absorption spectroscopy and computer simulation [41]. Lattice energy minimisation calculations [42] were carried out in which extra-framework sodium and potassium ions were introduced into the model structure on different sets of randomly-distributed positions. The structures were then optimised subject to the constraint of the original model symmetry [38], and those with the lowest lattice energy were then further minimised without regard to any internal symmetry. The most notable feature of these calculations was the wide range of Ti-O bond distances which emerged. These simulated structures, including the alkali cation locations, were used as the basis for interpretation of both XANES and EXAFS spectra (recorded using the Ti Kedge) which had initially provided contradictory evidence, XANES suggesting six-fold coordination of Ti and EXAFS four-fold. H o w e v e r when multiple scattering effects were into account, the EXAFS spectra were able to be u n d e r s t o o d in terms of a distorted octahedral TiO 6 e n v i r o n m e n t , with alternating long and short Ti-O distances (respectively 2.11 and 1.71~) along the Ti-O-Ti chain direction, and four bonds of intermediate length (2.02~) in the TiO-Si linkages. The Ti-O-Ti bond angle was around 165 ~ This geometry, shown in Figure 2, is more reasonable than that originally proposed [38], in which the Ti-O-Ti chains were almost linear, in that it is comparable to that found in other chain titanate materials notably the non-linear optical material KTiO(PO 4) known as KTP [43-44].
Si i
Ti f~t
2.11
~::~---~
~
l o ~~'~ 2~2//
Ti ~. / 2 . 0 2
d'~
2.11 \
\
~
({ o ~
~_~4
Ti
_
~
--
~ :
x.~
~.,
1.82
165 ~
C)Si
Figure 1. Ti environment in ETS-10.
Figure 2. Calculated Fe geometry in Fe-ZSM-5.
Diffusion in zeolites Two complementary approaches are available for modelling the diffusion of molecules in the pores of microporous materials. The most direct is v i a the 3.2.
92 use of the Molecular Dynamics (MD) technique which allows diffusion coefficients to be obtained from the mean square displacements of molecules as a function of time; the method is, however, limited to rapidly diffusing species. In contrast, for slower migration we can use the transition state theory approach which requires the identification of saddle points for the migration process. Recent examples of both are discussed below. 3.2.1. MD simulation of n-butane and n-hexane in silicalite A recent detailed study of this problem was reported by Hernandez [45] using long time scale (1000ps) dynamical simulations. The calculated diffusion coefficients are reported in Table 1. As discussed in reference [45], these are in good agreement with experimental data. Table 1 Diffusion coefficients of n-butane and n-hexane in silicalite as a function of system temperature at a loading of 4 molecules/u.c.
(Ta)
Dtot
(K)
n-butane
n-hexane
Dx
Dy
Dz
(cm2s-lxl05)
(cm2s-lxl05)
(cm2s-lxl05)
209.4
0.93(2)
0.45(2)
2.23(2)
0.109(2)
287.2
2.93(2)
1.71 (2)
6.65(2)
0.415(3)
400.1
4.15(2)
3.75(2)
7.70(4)
0.980(4)
206.6
0.56(1)
0.123(6)
1.555(3)
0.0235(8)
314.1
1.42(2)
0.69(1)
3.42(4)
0.160(2)
380.8
2.17(1)
1.28(2)
4.45(3)
0.383(2)
The simulations also were able to provide insight into the mechanism of molecular migration. From analysis of individual trajectories it was clear that diffusion takes place by means of jumps, i.e. by means of a hopping mechanism. The molecules remain trapped for long times in potential energy minima located at the channel sections, and eventually gain sufficient energy to overcome the potential energy barriers posed by the channel intersections. When this happens the molecule undertakes a rapid jump which is completed in just a few ps, reaching a new minimum. It was observed that at intermediate loadings (4 molecules/u.c.) the jump lengths were of the order of 10~ for both n-butane and n-hexane, which corresponds roughly to the distance between channel sections across intersection regions, which is in good agreement with the average jump lengths determined from neutron scattering experiments by Jobic et al. [46]. Further details are again available in reference [45]. 3.2.2. Transition state approach to hydrocarbon diffusion in DAF-1 Despite the success and value of MD techniques, they are, as noted above, inherently limited in that the number of diffusion events may be insufficient
93 during the 'real time' sampled by these simulations. In these cases, which occur with more slowly diffusing species, then a transition state theory becomes more appropriate, with the transition state being identified by a form of constrained minimisation [47]. In this method, the diffusion pathway, or at least an initial trajectory, is pre-defined and a series of energy minimisation calculations is carried out at close intervals as the molecule moves in a stepwise fashion along a proposed migration trajectory. Thus the minimum energy profile may be obtained. In a recent study [48] this method was applied to the diffusion of the four isomers of butene in the microporous aluminophosphate DAF-1. This framework contains two separate parallel channel systems defined by 12-ring pores. One of these is one-dimensional, while the other consists of a threedimensional network of channels, cross-linked by smaller 10-ring pores. The two channel systems are connected to each another by only by 8-ring pores. It was found that the butene molecules were able to access the entire network of the three-dimensional channel system, with the highest diffusion barriers lying in the range 17 to 22 kJmo1-1. However none of the isomers wer(~ able to pass between the two distinct channel systems, thus rendering them completely independent. The migration route identified by the calculation is shown in Figure 3.
I u
Figure 3. Calculated diffusion trajectory of isobutene between the double 10rings in DAF-1 together with the associated energy profile.
3.3
Template-Host Interactions The use of organic bases in the synthesis of microporous materials as structure-directing agents or templates is widespread. Indeed, of all the factors influencing the formation of microporous structures, it is this templating action
94 that appears to be the most likely to allow access to, and control over, new structural types, particularly in the aluminophosphate family of materials. Moreover, the current focus of attempts at designing new materials is on the selection of templates which have specific features which are expected to be reflected in any structure formed [49]. However, the exact function of templates is not understood and the extent to which they are critical to the formation of such materials under debate [50]. In order to establish whether this effect can be quantified in any way and to determine if computational methods can be applied to design new microporous materials, we have studied extensively the interactions of large range of templates and framework types [48, 51]. In order to locate templates in frameworks and to determine their interactions we have applied the methodology of Freeman et al. [4] which, as we have noted, is based on a combination of molecular dynamics, Monte Carlo and energy minimisation techniques. For a selected molecule, a library of conformations are generated using molecular dynamics, which are then docked into a framework using a Monte Carlo procedure. Suitable conformations are accepted according to a supplied energy cut-off and subsequently energy minimised producing a library of low energy configurations. We have shown that the method can successfully locate templates at experimentally determined positions [48, 51], in studies of cyclic templates in NU-3, tetrapropylammonium in ZSM-5 as well as in simulation of the postulated positions of tri-quaternary amine used in ZSM-18 synthesis and for hexamethonium in EU-1. Furthermore we have demonstrated a correlation between the ability of a template to form a particular framework with the nonbonding interactions of that template with the framework, as demonstrated in Figure 4 and further in Table 2 where the technique is successful at selecting the correct template for a given framework. Simulations of this type can therefore provided a quantification of the experimentally noted "good fit" of templates in the frameworks they form [52]. The crucial r61e of non-bonding interactions between the framework and the template is further emphasised by the ability of the technique to distinguish subtle effects such as small changes in unit cell parameters. For example, zeolite NU-3, when synthesised with two different cyclic templates, forms with unit cell parameters that are noticeably different (by -1.5%) [53]. Calculations (Table 3) show that the most stable template / unit cell combinations are those that are found experimentally. Furthermore, the template which best matches that of the hydrated calcium ion found in the natural analogue Levyne [54] has a higher binding energy in the unit cell of the mineral form. These results provide a basis on which we may now begin to attempt to apply computational methods in assisting the synthesis of new materials. The success of this work will, furthermore, allow us to probe further the nature of templating and the synthesis of microporous materials in general; a correlation between crystallisation rate and template-framework interactions has also been demonstrated using similar computational methods [55].
95 Table 2 a) Non-bonded interactions energy of tetraalkyl ammonium cations in various siliceous frameworks. Templates predicted as effective are emboldened. *Experimental template. b) Packing energy, i.e. the interaction between template molecules, of tetraalkyl ammonium template / framework combination when two adjacent template molecules are included. From these two figures, we can select the most suitable template for each framework. i
a) ZSM-5
ZSM-11
Einter (kJ mo1-1)
Einter (kJ mo1-1)
Einte r (kJ tool -1)
TMA
-51.7
TMA
-38.7
TMA
-43.1
TEA
-92.1
TEA
-73.0
TEA*
-104.7
TPA*
-133.9
TPA
-119.9
TPA
-83.4
TBA
-165.5
TBA*
-159.5
TBA
-56.7
i
b)
Template / framework
AEpack (kJ mo1-1)
TPA / ZSM-5
-29.7
TBA / ZSM-5
+14.9
TBA / ZSM-11
-18.3
TPA / ZSM-11
-8.5
Table 3. The interaction energies of the templates N-methylquinuclidinium (N-MeQ) and 1-aminoadamantane (AmAdam) in the different LEV unit cells. Framework (template)
Lattice parameter (A) a
NU-3 (N-MeQ) [53]
NU-3 (AmAdam) [53]
Levyne [54]
13.0595
13.2251
13.338
Template
Einter / kJ mo1-1
N-MeQ
-96.3
AmAdam
-94.4
AmAdam
-95.4
N-MeQ
-90.0
AmAdam
-90.1
N-MeQ
-92.1
c
22.6061
22.2916
23.014
96
---e--- tetraalkylammonium cations A bis-quaternary amines v c~0-diamines [] saturated cyclic • unsaturated cyclic -40
9
V
=
-80 E / ld mol
-1 r A&
-120-
-160-
I
50
'
I
100
'
I
150
'
I
200
'
I
250
'
Molecular Volume / ~ 3 Figure 4. Interaction Energy of experimental framework / template combinations as a function of molecular volume. Straight line is the best fit through all datapoints. Although the overall correlation shows considerable scatter, if single homologous series are considered then the correlation between template size/shape and interaction energy is excellent, as is evident for the tetraalkylammonium cations (highlighted with a line) and the c~,c0-diamines. 3.4.
Acid site-methanol interactions There has been much debate concerning the nature of the adsorbed state of methanol at Bronsted acid sites within microporous materials, in particular the question of whether there exists a chemisorbed complex in which the proton is transferred from the framework to form the methoxonium cation. We have performed ab initio gradient corrected density functional calculations to examine this question based on cluster models containing both three and four tetrahedral sites (H3SiOHAI(OH)2OSiH3 and H3SiOHAI(OH)(OSiH3)2 respectively). The physisorbed complex of methanol, in which two hydrogen bonds are formed with the acid site, is found to be the most stable configuration with a binding energy of 64.1 and 58.3 kJmo1-1 for the Becke-Perdew (BP) and Becke-
97 Lee-Yang-Parr (BLYP) functionals in good agreement with the lower bound of experimental estimates. No minimum exists corresponding to the chemisorbed (protonated) species and this complex corresponds to a transition state for methanol mediated proton exchange between framework oxygens. The BeckePerdew functional closely reproduces the geometry of the physisorbed complex obtained by Haase and Sauer [17] at the MP2 level. Detailed results for the 3T cluster model are given in Table 4 Table 4 Properties of methanol adsorbed on the 3T cluster model for BP and BLYP gradient corrected functionals, with the Hartree Fock and MP2 results of Haase and Sauer [17] included for comparison (Ore = oxygen of methanol, Hm = h y d r o g e n of methanol, 02 = zeolite oxygen of OH group coordinated to methanol, Oz' = oxygen of zeolite hydrogen bonding to Hm). |l
i|
BP
BLYP
HF [17]
MI~ [17]
Binding energy (kJmol-1) *
69.86
63.75
49.4
79.0
r ( O m - Hm) (]~)
1,009
1.001
0.953
0.993
r(Om - C) (]~)
1.449
1.460
1.404
1.425
r(Oz - Hz) (]k)
1.051
1.035
0.971
1.033
r ( O m - Hz) (]k)
1.498
1.569
1.734
1.499
r(Oz' - Hm) (]~)
1.727
1.837
2.166
1.737
r(A1 - Oz) (]k)
1.931
1.945
1.904
1.896
Z(Hz - Oz - A1) (o)
110.49
110.95
Z ( H m - O r e - C) (o)
109.46
109.18
* Values prior to correction for zero point energy. ZPE correction for BLYP = 5.43 kJmo1-1. Calculated vibrational frequencies for this complex alone are unable to rationalise the experimental infra red spectra. However, large shifts are predicted for the framework hydroxyl to 2442-2675 cm -1, depending on the functional used, which accords with the observation of a broad band at 2400cm -1 when allowing for the fact that larger cluster models will further lower the calculated frequencies. Preliminary calculations have been performed to examine the effect of increasing the loading of methanol to two molecules per acid site. The a d d i t i o n a l m e t h a n o l molecule fails to stabilise the f o r m a t i o n of the m e t h o x o n i u m ion and the m i n i m u m energy configuration contains the two
98 molecules in an eight membered hydrogen bonded ring. The heat of adsorption for the second molecule is found to be only 8 kJmo1-1 less than that for the first. Although no evidence was found for the formation of a methoxonium ion within the framework of cluster calculations, a parallel s t u d y based on periodic boundary conditions for methanol in chabazite indicates that this may in fact be the stable species when long range interactions are taken into consideration [56]. 4.
CONCLUSIONS AND FUTURE DIRECTIONS This brief review has, we hope, illustrated the diverse range of problems that can now be investigated by computer modelling techniques. The future of the field will involve accurate and precise 'forcefield' calculations on highly complex systems using reliable parameterisations; and high level quantum mechanical calculations on reaction mechanisms. The c o n t i n u i n g developments in both hardware and software will lead to an increasingly prominent r61e for computational techniques in zeolite science. 5.
ACKNOWLEDGEMENTS We are grateful to J.M. Thomas, C.M. Freeman, M.J. Anderson, S.W. Carr, E. Hernandez, P. Voigt, J. Sauer and R.A. van Santen for contributions to and discussions concerning this work. We wish to thank BIOSYM Technologies, Unilever and EPSRC for their support. REFERENCES
1. 2. 3. 4. 5. 6. 7. 8.
C.R.A. Catlow (ed.), Modelling of Structures and Reactivity in Zeolites. Academic Press, London 1992. C.J. Kramer, R.A. van Santen, C.A. Emeis, A.K. Nowak, Nature, 363 (1993) 529. J. Sauer, Struc.Surf.Sci.Catal., 84 (1994) 2039. C.M. F r e e m a n , C.R.A. Catlow, J.M. Thomas and S. Brode, Chem.Phys.Letts. 186 (1991) 137. M.J. Sanders, M. Leslie and C.R.A. Catlow, J.Chem.Soc., Chem.Comm., 1271 (1994). B.W.H. van Beest, G.J. Kramer, R.A. van Santen, Phys.Rev.Lett., 64 (1990) 1955. J.M. Purton, R. Jones, C.R.A. Catlow and M.Leslie, Phys.Chem.Minerals, 19 (1993) 392. C.R.A. Catlow, J.M. Thomas, C.M. Freeman, P.A. Wright and R.G. Bell, Proc.Roy.Soc. A, 442 (1993) 85
9. 10.
N.J. Henson, A.K. Cheetham, J.D. Gale, Chem.Mater., 6 (1994) 164. E.D. de vos Burchart, H. van Bekkum, B. van der Graaf, J.Chem.Soc., Faraday Trans., 88 (1992) 2761.
11. 12.
J.R. Hill, J. Sauer, J.Phys.Chem., 98 (1994) 1238. R.A. Jackson, C.R.A. Catlow, Mol.Sim., 1 (1988) 207.
99 13. 14. 15. 16. 17. 18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30. 31. 32.
33. 34. 35. 36. 37. 38.
A.V. Kiselev, A.A. Lopatkin, A.A. Shulga, Zeolites, 4 (1985) 261. Solids_docker, version 5.0, BIOSYM Technologies Inc., San Diego, 1994. J. Sauer, P.Ugliengo, E. Garrone and V.R. Saunders, Chem.Rev., 94 (1994) 2095. J.D. Gale, C.R.A. Catlow and J.R. Carruthers, Chem.Phys.Lett., 216 (1993) 155. F. Haase and J. Sauer, J.Amer.Chem.Soc., 117 (1995) 155. M. Allarena, K. Seito, E. Kassalo, Gy Ferenczy and J.G. Angyan, Chem.Phys.Lett., 168 (1990) 461. S. Greatbanks, P. Sherwood and I.H. Hillier, J.Phys.Chem., 98 (1994) 8134. J.C. White and A.C. Hess, J.Phys.Chem., 97 (1993) 8703. P. Rathnasamy, R. Kunar, Catal.Today, 9 (1991) 329. D.W. Lewis, C.R.A. Catlow, G. Sankar, S.W. Carr, J.Phys.Chem., 99 (1995) 2377. S.A. Axon, K.K. Fox, S.W. Carr, J. Klinowski, Chem.Phys.Lett., 189 (1992) 1. J.S. Reddy. R. Kumar, P. Ratnasamy, Appl.Catal., 58 (1990) L1. D.V. Serrano, H-X. Li, M.E. Davis, J.Chem.Soc., Chem.Commun. (1992) 745. M.A. Camblor, A. Corma, A. Martinez, J.Chem.Soc., Chem.Commun., (1992) 589 A. Corma, M.T. Navarro, J. P6rez Pariente, J. J.Chem.Soc., Chem.Commun., (1994) 147. T. Tatsumi, M. Nakamura, S. Negishi, M. Tominaga, J.Chem.Soc., Chem.Commun., (1990) 476. D.R.C. Huybrechts, L. De Bruycker, P.A. Jacobs, Nature 345 (1990) 240. D.M. Poojary, R.A. Cahill, A. Clearfield, Chem. Mater. 6 (1994) 2364. A. Jentys, C.R.A. Caflow, Catal Lett. 22 (1993) 251. S. Bordiga, S. Coluccia, C. Lamberti. L. Marchese, A. Zecchina, F. Boscherini, F. Buffa, F. Genoni, G. Lepfanti, G. Petrini, G. Vlaic, J.Phys.Chem. 98 (1994) 4125 T. Blasco. M.A. Camblor, A. Corma, A. Perez-Pariente, J.Amer.Chem.Soc. 115 (1993) 11806. G. Sankar, F. Rey, J.M. Thomas, G.N. Greaves, A. Corma, B.R. Dobson, A.J. Dent,J.Chem.Soc., Chem.Commun., (1994) 2279. S.M. Kuznicki, US Patent No. 4853202 (1989) S.M. Kuznicki, A.K. Thrush, European Patent No. 04005978A1 (1990) D.M. Chapman, A.L. Roe, Zeolites, (1990) 10, 730 M.W. Anderson, O. Teraski, T. Ohsuna, A. Phillppou, S.P. MacKay, A. Ferreira, J. Rocha, S. Lidin, Nature 387 (1994) 347.
100 39. 40. 41. 42. 43. 44. 45. 46.
47. 48.
49. 50. 51. 52. 53. 54. 55. 56.
T. Ohsuna, O. Terasaki, D. Watanabe, M.W. Anderson, S. Lidin, Stud.Surf.Sci.Catal., 84 (1994) 413. M.W. Anderson, O. Terasaki, T. Ohsuna, P.J. O'Malley, A. Philippou, S.P. MacKay, A. Ferreira, J. Rocha, S. Lidin, Phil.Mag. B, in press. G. Sankar, R.G. Bell, J.M. Thomas, M.W. Anderson, P.A. Wright & J. Rocha, to be published R.A. Jackson, S.C. Parker, P. Tschaufeser in Modelling of Structures and Reactivity in Zeolites. C.R.A. Catlow (ed.), Academic Press, London 1992. N.K. Hansen J. Protas. G. Marnier. Acta.Cryst.B 47 (1991) 660. M.M. Eddy, T.E. Gier, N.L. Keder, G.D. Stucky, D.E. Cox, J.D. Bierlein, G. Jones, Inorg.Chem. 27 (1988) 1856. E. Hernandez and C.R.A. Catlow, Proc.Roy.Soc., 448, (1995) 143. H. Jobic, M.Bee and J. Caro, Proc. 9th Int. Zeolite Conf, (eds. R. von Balmoos, J.B. Higgins and M.M.J. Tracy) Butterworth-Heinemann, Boston, 1993. GCMC Solid Docker Module, verion 5.0, BIOSYM Technologies Inc., San Diego, 1994. R.G. Bell, D.W. Lewis, P. Voigt, CM Freeman, J.M. Thomas, CRA Catlow Stuc Surf Sci Catal, 84, 2075 (1994). S.I. Zones, M.N. Olmstead, D.S. Santilli, Journal of the American Chemical Society, 164 (1992) 4195. Davis, M. E.; Lobo, R. F. Chemistry of Materials 4 (1992) 759. D.W. Lewis, C.M. Freeman, C.R.A. Catlow, Journal of Physical Chemistry 1995, in press, H. Gies, B. Marler, Zeolites 12 (1992) 42. L.B. McCusker, Materials Science Forum 423 (1993) 133-136. S. Merlino, E. Galli, A. Alberti, Tschermaks Mineral. Petrogr. Mitt. 22 (1975) 117. T.V. Harris, S.I. Zones, Struc.Surf.Sci.Catal., 84 (1994) 29. R. Shah, J.D. Gale, M.C. Payne and V. Heine n manuscript in preparation.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 1995 Elsevier Science B.V.
101
Computational studies of water adsorption in zeolites S. A. Z y g m u n t a, L. A. C u r t i s s b, a n d L. E. Iton b aDepartment of Physics and Astronomy, Valparaiso University, Valparaiso, IN 46383 (email:
[email protected]) bArgonne National Laboratory, curtiss @ cmt.anl.gov)
Argonne,
IL
60439
(email"
We have performed high-level ab initio calculations using Hartree-Fock (HF) theory, Mr perturbation theory (MP2), and density-functional theory (DFT) to study the geometry and energetics of the adsorption complex involving H 2 0 and the BrCnsted acid site in the zeolite H-ZSM-5. These calculations use aluminosilicate cluster models for the zeolite framework with as many as 28 T atoms (T=Si,A1). We included geometry optimization in the local vicinity of the acid site at the MP2 and DFT levels of theory for the smallest cluster, while in the larger clusters this was done at the HF/6-31G(d) level of theory. We have also calculated corrections for zero-point energies, extensions to higher basis sets, and higher levels of electron correlation. Results for the adsorption energy and geometry of this complex are reported and compared with previous theoretical and experimental values.
1. I N T R O D U C T I O N BrCnsted acid chemistry is a dominant feature of the catalysis by zeolites in many important industrial applications. A reliable theoretical treatment of the proton affinity of H-ZSM-5 zeolite has been obtained in previous work using high-level ab initio calculations on large cluster models [1]. Proton transfer to a strong adsorbed base has also been studied theoretically in the interaction of ammonia with the BrCnsted acid site [2-4]. The interaction of weak bases, e.g., H 2 0 , presents a more equivocal situation. What kind of equilibrium structure is formed when H 2 0 is adsorbed at the Brr acid site in H-ZSM-5? Some e x p e r i m e n t a l evidence, most notably in the form of IR spectroscopy, has suggested that the acidic proton is transferred to H 2 0 and that an ion-pair structure is most stable [5,6]. One ab initio theoretical study [7] also gave evidence to support this conclusion. However, recent ab initio calculations have disputed this claim and have led to a reinterpretation of the IR spectra in a manner consistent with a neutral hydrogen-bonded adsorbate [8,9]. These studies have suggested that the ion-pair complex should be regarded as a transition state and not a true equilibrium geometry. However, almost all of these theoretical studies have used small clusters to represent the acid site, and none have accounted for electron correlation in their optimization of molecular geometries, so they are open to criticism on the basis of these limitations.
102
The calculations presented here extend our earlier study of the adsorption of H 2 0 on a 2 T atom cluster model of H-ZSM-5 [10]. They incorporate local geometry optimization, large cluster size, and electron correlation in a unified way. We have obtained results for the geometry and adsorption energy of the neutral H 2 0 adsorption complex in H-ZSM-5, and have found that it is more stable than the ion-pair structure. The calculated adsorption energy is roughly consistent with the published experimental value. 2. T H E O R E T I C A L M E T H O D S The theoretical calculations presented here are based on ab initio molecular orbital theory [11,12] and density-functional theory [13]. We used four aluminosilicate clusters of increasing size to model the BrCnsted acid site in HZSM-5. These clusters include 3, 8, 18, and 28 T atoms, and have a total number of 14, 34, 69, and 101 atoms, respectively. Each cluster includes one A1 atom and a c h a r g e - b a l a n c i n g proton to maintain a neutral zeolite framework, and is terminated by H atoms at the periphery. Their stoichiometries are H 9 S i 2 A 1 0 2 , H 1 9 S i 7 A 1 0 7 , H 2 9 S i 1 7 A 1 0 2 2 , and H 3 3 S i 2 7 A 1 0 4 0 , respectively. For the 3 T atom cluster, the adsorption complex was found by using full geometry optimization. This allowed us to calculate zero-point vibrational energy corrections directly. These corrections were then used as estimates for the complexes between H 2 0 and the larger cluster models. For the 8 T atom cluster, the constant-volume relaxation (CVR) method [1] was used. Atoms at the periphery of the cluster were fixed at positions determined from x-ray diffraction studies of H-ZSM-5 [14], while the central 0 3 S i O H A 1 0 3 atoms near the acid site were fully relaxed. In addition, the six intermolecular degrees of freedom between the framework and the adsorbate molecule were fully optimized. The H 2 0 and H3 O+ geometries were held fixed at the optimized geometries of the isolated molecules. This constrained relaxation scheme is a useful model for the effect of an adsorbate on the local structure of the acid site. After CVR optimization, the effect of more distant atoms was then included by embedding this 8 T atom cluster in successively larger fragments of crystalline H-ZSM-5 to obtain first the 18 T atom and then the 28 T atom cluster. This procedure yielded a cluster size energy correction term. Our procedure is open to the criticism that the intermolecular degrees of freedom were not re-optimized in the 18 and 28 T atom clusters, but we tested its accuracy by re-optimizing the intermolecular coordinates of the 18 T atom complex with H 3 0 + at the HF/3-21G level and comparing them to those obtained in the 8 T atom cluster. Changes in bond lengths and angles on the order of 3-5 % were noted, but the total energy after re-optimization decreased by less than 1 kcal/mol, so we believe that this procedure is justified. Both 3-21G and 6-31G(d) basis sets were used in the calculations involving the 8, 18, and 28 T atom clusters, while in the 3 T atom cluster an additional calculation was performed with the 6-311+G(3df,2p) basis set. This result for the smallest cluster model allowed us to find a basis set energy correction, which was then used as an estimate for the larger clusters based on G2(MP2) theory [15]. In the 3 T atom cluster, the effect of electron correlation was treated by MP2 theory, the non-local BLYP formulation of DFT [16], and quadratic configuration interaction (QCISD(T)) [17]. These results allowed us to find correlation energy corrections which were used as estimates for the larger clusters. They also
103
provided a test of the accuracy of MP2 theory and BLYP more computationally demanding QCISD(T) method. 3. R E S U L T S
AND
when
compared
to the
DISCUSSION
The reaction energies of H 2 0 i n t e r a c t i n g at the h y d r o x y l site of aluminosilicate clusters of 3, 8, 18, and 28 T atoms representing H-ZSM-5 are listed in Tables 1 and 2. The quantities calculated in this study include A E i o n , A E c o v , AErel, and AEdesorp. The AEion is the complexation energy of the ionic complex
(1)
AEion = E(Z-) + E(H3 O+) - E(Z-...OH3 +) where
Z- is the unprotonated zeolitic cluster and Z-....OH3 + is the ion-pair complex.
Table 1 H 2 0 reaction energies, AEcov and AEion (in
kcal/mol), for different cluster sizes a
AEcov
AEion
Method/Basis
3
8
18
28
3
8
18
28
HF/3-21G
-
31.7
34.8
34.2
-
154.6
154.2
154.6
HF/6-31G(d)
15.2
14.7
17.0
16.7
138.4
131.1
130.9
129.7
MP2/6-31G(d) b
22.1
20.2
-
-
150.1
138.1
-
-
aAll results are from the constant volume relaxation procedure as described text, except for cluster 3, which is a full geometry optimization. Cluster 3 is illustrated in Figure 1. Zero-point energies not included in values. bAt HF/6-31G(d) geometry for cluster 8.
Table 2 H 2 0 reaction energies, AErel and AEdesorp (in
kcal/mol), for different
in
cluster
sizes a
AErel
AEdesorp
Method/Basis
3
8
18
28
3
8
18
28
HF/3-21G
-
-14.1
-13.0
-10.4
-
31.7
34.8
34.2
-14.5
-16.9
-14.7
-13.3
15.2
14.7
17.0
16.7
-6.2
-12.4
-
-
22.1
20.2
-
-
HF/6-31G(d) M P 2 / 6 - 3 1 G(d) b -i
i-
aAll results are from the constant volume relaxation procedure as described text, except for cluster 3, which is a full geometry optimization. Cluster 3 is illustrated in Figure 1. Zero-point energies not included in values. bAt HF/6-31G(d) geometry for cluster 8.
in
104
The AEcov
is the complexation energy of the covalent (hydrogen-bonded) complex
(2)
AEcov = E(ZH) + E(H20) - E(ZH...OH2)
where ZH is the protonated zeolitic cluster and ZH .... OH2 is the covalent complex. The AErel is the energy difference between the covalent and ionic complexes
(3)
AErel = E(ZH...OH2) - E(Z-...OH3 +)
where a positive value indicates that the ionic complex is more stable. The AEdesorp is the energy required to remove the H 2 0 molecule from the most stable complex (ionic or covalent) AEdesorp = E(ZH) + E(H20) - min[E(Z-...H30+), E(ZH...OH2)]
(4)
The results in Tables 1 and 2 for these energies are based on calculations which include relaxation of the local region of the cluster near the hydroxyl site as described in the previous section. Results for the 3 T atom cluster, for which full optimizations were carried out, are also included in the table. The structures of the ion-pair and hydrogen-bonded configurations for the 3 T cluster are illustrated in Figure 1. A comparison of the calculated geometrical parameters at HF, MP2, and BLYP levels of theory using the 6-31G(d) basis set is shown in Table 3. At all these levels, the ion-pair structure is a transition state, while the covalent structure is a local minimum in the potential energy surface. In Table 3 note p a r t i c u l a r l y the significant influence of electron c o r r e l a t i o n on the h y d r o g e n - b o n d distances OH1 and OH2 in the covalent complex. Complexation energies for both structures are also strongly influenced by correlation. Also note that MP2 and BLYP give very similar results for the covalent structure.
('~
OH 9
', OH
.s
l
(a)
~
(~
,~, OH1 "'"
OH2 ""
sSa
(b)
Figure 1. Optimized structures of (a) ion-pair and (b) hydrogen-bonded (covalent) configurations for H 2 0 interacting with the hydroxyl site in an aluminosilicate cluster with three T atoms.
105
Table 3 Structure and Energetics of 3 T Atom Clusters at Various Levels of Theory (see Figure 1 for explanation of coordinates) a
HF/6-31G(d)
MP2/6-31G(d)
1.42 96.8 138.4
1.36 95.4 150.1
OH 1 OH 2 OAIO AEco v
2.01 1.75 98.5 15.2
1.81 1.61 97.2 22.1
1.76 1.56 97.2 22.3
AEre I
-14.5
-6.2
-4.0
ion-pair
structure
OH OAIO AEio n covalent
aBond
BLYP/6-31G(d)
structure
lengths in /~, angles in degrees, and energies in kcal/mol.
The HF/6-31G(d) calculations for the 8 T atom cluster also show that the lowest energy structure is a h y d r o g e n - b o n d e d adsorption complex between H 2 0 and the zeolite framework, in which the adsorbate is anchored to the framework by O...H linkages of 1.70 and 2.06 /~. These bond lengths are within 0.05 /~ of the HF results for the 3 T atom cluster shown in Table 3, and they are nearly the same as those found in a previous study [18] using a slightly different DZP basis set and a smaller 3 T atom zeolite cluster. The adsorbed complexes ZH...OH2 and Z-...OH3 + are shown in Figure 2 for the 8, 18, and 28 T atom clusters. The terminating H atoms at the periphery of these clusters are not shown in the figure. Table 4 shows our energy corrections to the calculated desorption energy of 14.7 kcal/mol in the 8 T atom cluster. Extending the cluster size to 28 T atoms [A(CS)] i n c r e a s e d the binding energy by 2.0 kcal/mol, and treating electron correlation in the 3 T atom cluster by MP2 theory [A(MP2)] gave an additional increase of 6.9 kcal/mol. Correlation effects beyond the MP2 level using the 631G(d) basis [A(QCI)] decreased the desorption energy by 0.9 kcal/mol in the 3T cluster. The zero-point energy correction [A(ZPE)] from the 3 T cluster gave a 2.9 kcal/mol decrease in desorption energy, and the correction from G2(MP2) theory for extension to a higher-level 6-311+G(3df,2p) basis set [A(BS)] gave an additional 5.5 kcal/mol decrease. This gives a best estimate of 14.3 kcal/mol for the desorption energy of H 2 0 in H-ZSM-5 at 0 K. Thermal effects will cause this value to decrease, but it is unclear if the usual ideal gas corrections used in theoretical enthalpy calculations [19] are valid in the restricted environment of the zeolite interior.
106
(a)
(c)
(e)
(b)
(d)
(f)
Figure 2. Z-...OH3 + and ZH...OH2 complexes for cluster size 8 (a,b), 18 (c,d), and 28 (e,f). Terminating H atoms not shown.
107
A previous theoretical estimate [20] for the desorption energy in a 2 T atom cluster was 11.2 kcal/mol, but this approach included no correction terms besides A(MP2) and only allowed for a single O...H linkage between the ZH framework and the H 2 0 molecule. Our earlier study [10], using a similar cluster model but including A(MP2), A(QCI), and A(BS) corrections, gave a value of 10.8 kcal/mole. Other theoretical work using a 3 T atom cluster [7] resulted in a value of 14.8 kcal/mol, but it did not account for the A(CS), A(QCI), and A(BS) terms calculated here. By comparison, the experimental enthalpy of adsorption, which was obtained from a Clausius-Clapeyron analysis of p(T) data between 357 and 435 K for a coverage of less than one molecule per acid site, was found to be 12+1 kcal/mol [5]. The result presented here, in light of the necessary thermal corrections, is consistent with experiment.
Table 4 Energy Corrections to AEdesorp (in kcal/mol) from 8 T Atom Cluster
AEdesorp (HF/6-31G(d))
14.7
A(CS) A(MP2) A(QCI) A(ZPE)
2.0 6.9 -0.9 -2.9
~x(Bs)
-5.5
AEdesorp (best estimate)
14.3
4. C O N C L U S I O N S Using aluminosilicate cluster models of up to 100 atoms, we have carried out a computational study based on ab initio molecular orbital theory of adsorption of H 2 0 at the acid site in the H-ZSM-5 zeolite. The computations incorporate local geometry optimization, large cluster size, and electron correlation in a unified way. The results indicate that the neutral H 2 0 adsorption complex is more stable than the ion-pair structure previously proposed, which is probably a transition state. The calculated adsorption energy is roughly consistent with the published experimental value. Our results show the usefulness of such computations in investigations of reactions at the acid site in zeolites. It is also evident that the MP2 and the BLYP methods give correlation corrections for the desorption energy which are less than 1 kcal/mol from that of the more sophisticated QCISD(T) technique. Since the BLYP method can be i m p l e m e n t e d with a lower computational cost than MP2, it may be useful in future adsorption studies. ACKNOWLEDGMENTS This work was supported by the U. S. Department of Energy, Office of Basic Energy Sciences, Division of Materials Sciences, under Contract No. W-31-109ENG-38. We acknowledge a grant of computer time at the National Energy Research Supercomputer Center. Acknowledgment is also made to the Donors of
108
the Petroleum Research Fund, adminstered by the American Chemical Society, for partial support of this research (S.A.Z.). REFERENCES
1. H. V. Brand, L. A. Curtiss, and L. E. Iton, J.
Phys. Chem. 97 (1993) 12773.
2. H. V. Brand, L. A. Curtiss, and L. E. Iton, J. Phys. Chem. 96 (1992) 7725. 3. E. H. Teunissen, A. P. Jansen, and R. A. van Santen, J. Phys. Chem. 99 (1995) 1873. 4. J. Sauer, P. Ugliengo, E. Garrone, and V. R. Saunders, Chem. Rev. 94 (1994) 2095. 5. A. Ison and R. J. Gorte, J. Catal. 89 (1984) 150. 6. M. T. Aronson, R. J. Gorte, and W. E. Farneth, J. Catal. 105 (1987) 455. 7. J. C. Sauer, C. Kolmel, F. Haase, and R. Ahlrichs, in Proceedings of the Ninth International Zeolite Conference, (Montreal 1992) R. von Ballmoos et al., eds., Reed Publishing, Stoneham, MA, Vol. I (1993) 679. 8. A. G. Pelmenschikov and R. A. van Santen, J. Phys. Chem. 97 (1993) 10678. 9. F. Haase and J. Sauer, J. Phys. Chem. 98 (1994) 3083. 10. S. A. Zygmunt, H. V. Brand, D. J. Lucas, L. E. Iton, and L. A. Curtiss, J. Mol. Struct. (Theochem) 314 (1994) 113. 11. W. J. Hehre, L. Radom, J. A. Pople, and P. v. R. Schleyer, Ab Initio Molecular Orbital Theory. (John Wiley, New York) 1987. 12. Gaussian 92, M. J. Frisch et al. (Gaussian, Inc., Pittsburgh, PA 15106) 1992. 13. R. G. Parr and W. Yang, Density-Functional Theory of Atoms and Molecules (Oxford Univ. Press, New York) 1989. 14. H. van Koningsveld, H, Van Bekkum, J. C. Jansen, Acta Crystallogr. B43 (1987) 127. 15. L. A. Curtiss, K. Raghavachari, and J. A. Pople, J. Phys. Chem. 98 (1993) 1293. 16. P. M. W. Gill, B. G. Johnson, J. A. Pople, and M. J. Frisch, Chem. Phys. Lett. 197 (1992) 499. 17. J. A. Pople, M. Head-Gordon, and K. Raghavachari, J. Phys. Chem. 87 (1987) 5968. 18. J. Sauer, H. Horn, M. Haser, and R. Ahlrichs, Chem. Phys. Lett. 173 (1990) 26. 19. J. E. Del Bene, H. D. Mettee, M. J. Frisch, B. T. Luke, and J. A. Pople, J. Phys. Chem. 87 (1983) 3279. 20. E. Kassab, K. Seiti, and M. Allavena, J. Phys. Chem. 95 (1990) 9425.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviotand S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
109
Modeling of adsorption properties of zeolites A. Goursot, I. Papai*, V. Vasilyev and F. Fajula URA 418 CNRS, Ecole Nationale Sup6rieure de Chimie de Montpellier 8, Rue de l'Ecole Normale, 34053 Montpellier C6dex 1, France
1. INTRODUCTION It is well k n o w n experimentally that d e h y d r a t e d A or X zeolites adsorb nitrogen when a gas mixture containing N 2 and 0 2 circulates through their large pores. It has been shown that this effect of N2 concentration, which has been attributed to the interaction b e t w e e n the zeolite cations and the nitrogen quadrupole, is dependent on the nature of the counterions [1-3]. Indeed, A or X zeolites exchanged with lithium or calcium have been reported as much more efficient for N2 a d s o r p t i o n than Na zeolites [2, 3]. A l t h o u g h extensive experiments have been performed in this field, there has been, up to now, no fundamental study of the different adsorption properties of N 2 and 0 2 in zeolites. Our aim is thus to investigate how N 2 and 0 2 interact with different cations and to delineate how large is the role of a purely electrostatic effect in the adsorption process. To this end, the interactions of N 2 and 0 2 with a positive point charge, with isolated Na + or Li + cations, with their dimers and with a small model cluster of zeolite have been analysed and compared. Moreover, the role of the ionic nature of the zeolite structure around the adsorption cationic site has also been investigated, using the embedding of a large n e t w o r k of point charges. All these calculations are first-principle calculations based on density functional theory (DFT).
2. M O D E L S
AND METHODS
As a general notation for the investigated systems the two molecules (N 2 and 0 2) and the two cations (Li + and Na +) will be generally referred to as Y2 and X+, respectively. The systems which correspond to the interaction of Y2 molecules with a positive point charge (q+) and with X+ will be denoted as q+Y2 and X+Y2. Those including the pentameric zeolite model will be denoted as m(X+)Y2 .
* permanent address : Institute of Isotopes of the Hungarian Acacademy of Sciences, H-1525 Budapest, P.O.B. 77, Hungary
110 Since the linear geometry was proven to be the most stable (cf. 3.1), the potential energy curves for X+Y2 (q+Y2) were obtained by varying the X-Y (q-Y) distance in the linear X...Y-Y arrangement with a Y-Y bond length fixed at the equilibrium value of the free Y2 molecules. These curves have been fully corrected for basis set superposition error (BSSE). The small zeolite cluster (Figure 1) we have chosen does not represent any specific site of zeolite X. Its use was necessary in order to analyse the role of the zeolite framework in the interaction between a cation and the N2 or 0 2 molecule. It also allowed to verify the replacement of the zeolite by a network of point charges. In this m(X +) cluster, the dangling bonds of the four Si a t o m s are saturated with H atoms with a fixed Sill bond distance of 1.50 A, and the Sill bonds are aligned with the corresponding SiO bonds of the X-ray structure of zeolite X [4]. The geometries of the m(X +) clusters have been optimized as described previouly [5]. Y2 was then approached to X+ in the OXO plane in a linear B-X...Y-Y arrangement, where B is the midpoint of the two oxygen atoms bonded to X+. Varying only the X-Y distance (r(X-Y)), i.e. fixing the geometry of the m(X +) clusters and the Y2 molecules at their equilibrium structure, the interaction energy has been evaluated as a function of r(X-Y). The BSSE corrections were calculated in the same way as for the X+Y2 systems. Assuming that the long range interactions were essentially electrostatic, Li+-N2 and Li+-O2 interaction energies were estimated when Li + was positionned either in a site II or in a site III of a faujasite framework and embedded in a network of point charges representing the atoms of 27 unit cells (18143). The point charges used for these calculations were +1.0, +1.245, +1.897, -1.0355 for Li, A1, Si and O centers, respectively. These values have been obtained through a fitting of the electrostatic potential of several model clusters of zeolite. The density functional calculations were performed within the LCGTO-DF formalism [6-8] using the deMon program package [9-11]. All the calculations, except for the geometry optimization of the m(X +) clusters was carried out at a nonlocal level, using Becke's exchange [12] and Perdew's correlation [13] functionals. Geometry optimization was performed at the local level of theory using the Dirac exchange term and the Vosko-Wilk-Nusair parameterization [14] for the correlation energy. The basis sets used are described in Ref. 5 and 15. The energy of the interaction of the Y2 molecules with one or several point charge(s) is calculated by including the related electrostatic terms in the Hamiltonian.
3. RESULTS AND DISCUSSION 3.1. Interaction of N2 and 0 2 with a point charge The interaction energies of N 2 and 0 2 with a single positive point charge in the linear arrangement are shown in Figure 2 as a function of the distance R between the point charge and the midpoint of the diatomic molecules. Although this model is an extreme simplification of the real Y2-zeolite interaction, the
111 fundamental principle of oxygen separation is clearly s e e n : the interaction energy of N 2 is significantly larger than that of 0 2, for the entire range of R. This trend can be easily related to the difference in the physical properties of N 2 and 0 2 molecules. Indeed, it follows from the general theory of long-range interactions [16] that the two leading terms in the interaction energy of a point charge and a h o m o n u c l e a r diatomic molecule are those associated w i t h the q u a d r u p o l e moment (0) (electrostatic term) and the dipole polarizability ((x) (induction term) of the diatomics. The angle d e p e n d e n t formulas for the electrostatic and induction energies are given by: OqR-3((3/2)cos2(l~1/2) and -(1/2)q2R -4(0c + (1/3)((x[ [- 0U_)(3cos2(D-1)), where R -- I R I; (Xll and c~J_ are the parallel and perpendicular component of the polarizability tensor; (x = (1/3)((x[ i + 2(X_L); (I) is the angle between the molecular axis of Y2 and the vector R pointing from the centre of mass of Y2 to the point charge. Since O has a negative value for N 2 and 0 2 , both terms are additive and contribute to the lower the total energy. Moreover, they reach their m a x i m u m absolute value for ~ =0., i.e. for a linear geometry. Considering the experimental values of O and 0[]} (O(N 2) = -1.093, 0 ( 0 2) =-0.299, (Xll (N2) = 14.75, (Xll (0 2) = 15.73 from Ref. 17, where both O and (Xll are in a. u.), one would expect the induction terms to be quite similar for N 2 and 0 2, whereas the quadrupole moments suggest that the electrostatic term is considerably larger for N2, resulting in favorable interaction energies for this molecule.
40
20-~ 0
O-
E
"
--~ -20 UJ
-40-60
~,,,i,,,~l~,,~l,,,
0
1
2
i,,,~1,,,,i,,
3
4
5
,
6
7
R (angs) Figure 1. The pentameric model cluster m(X+)Y2.
Figure 2. Potential energy curves of q+N2. (a) and q+O2 (b).
112 3.2. Interaction of N2 and 0 2 with Li + and Na + cations As expected from the results above, the geometry optimization yields linear structures for all four molecules. The equilibrium r(X-Y) distances are 2.19, 2.11, 2.62 and 2.56 A for Li+N2, Li+O2 , Na+N2 and Na+O2, respectively. The corresponding potential energy curves for X+N2 and X+O2 are displayed in Figure 3 and 4. The relevant parts of the q+N 2 and q+O 2 curves are also given for comparison. These curves have been evaluated for each system (including BSSE corrections), the r(Y-Y) distance being fixed at the equilibrium value of the free Y2 molecules (1.118 A for N 2 and 1.232 A for O2), which are very similar to those in the X+Y2 systems. Consistently with the results for q+Y2, Li+N2 is more stable than Li+O2 and Na+N2 is more stable than Na+O2 . In addition, it is seen that the dissociation energies of the Li+Y2 systems are always larger than the corresponding Na+Y2 values. Moreover, we see that, for a given Y2, the Li+Y2 and Na+Y2 curves become identical for large distances ( R > 4 A ), and that, in this region, they fall very close to the q+Y2 curves. The X+-Y2 interaction is thus very well represented by the point charge model for distances sufficiently larger than the equilibrium distance. It appears that the reason why the Li+Y2 systems are thermodynamically more stable than the corresponding Na+Y2 systems is that the repulsive short range forces become significant at much shorter distances for Li + than for Na +, introducing larger electrostatic and induction energies in the total interaction energy. This explains the fact that, replacing Na + by Li + increases the binding energy with N2 (3.7 kcalmole -1) more than the binding energy with 0 2 (2.5 kcalmole-1), favoring the N2-O2 separation.
10
0
_
-$, ~-10 N
v
At p
v
LLI
.
o
/
o
/
W
r I
-20
o a
/
-10
9c
o a
d
A c
All
9
9 b
-30
I
1,5
'
-15
I
2,5 3,5 r(X-Y) (angs)
Figure 3. Potential energy curves of Na+N2 (a), Li+N2 (b) and q+N2 (c).
4,5
'
1,5
!
'
b !
2,5 3,5 r(X-Y) (angs)
'
4,5
Figure 4. Potential energy curves of Na+O2 (a), Li+O2 (b) and q+O2 (c).
113 Although N2 and 0 2 adsorption energies seem to differ essentially through the quadrupole dependent term, it is worth to investigate the relative weights of the electrostatic and induction contributions to their binding energies. With this purpose, we have considered the interaction of N2 and 0 2 with a Li+ dimer. The Y2 molecule can be situated either in a bridged geometry with each end bonded to a Li cation or in a top position, with one end bonded to a single cation. Several bridged structures have been optimized, for different Li-Li fixed distances. Their calculated geometries and binding energies (not corrected for BSSE) are presented in Table 1. These results show that the optimum Li-Li distance is 6.0 A for 0 2 and 5.5 or 6.0 ,a, for N2. In fact, these values correspond to distances between two cations located at site II and site III in the faujasite framework.
Table 1 Binding energies (B.E.) of N2 and 0 2 in bridged structures between two Li cations (distances in A, energies in kcal/mole) r(Li-Li)
r(Li-N)
B.E.(N2)
r(Li-O)
B.E.(O2)
5.3 5.5 6.0 6.5
2.10 2.20 2.45 2.70
12.3 13.2 13.1 11.5
2.05 2.15 2.40 2.65
2.8 4.0 5.1 4.8
The presence of the second Li cation, in these symmetrical structures, has a stabilizing effect, since it doubles the quadrupole energy term, but, at the same time, it has a destabilizing effect because the induced dipole created by symmetrically placed charges vanishes the induction term. A Y2 molecule on top on a Li + dimer has a preferred bent structure with a lowest energy for a (LiLlY) angle of around 160 ~ For a Li + - Li + distance of 6A, the corresponding binding energies are 15.2 and 10.9 kcal/mole for N2 and 02, respectively. The analysis of the binding energies with respect to different bending angles shows that these energy values are almost constant if the Y2 molecules approach the cation within a cone defined by a (LiLiY) angle of 110 ~ The binding energies will then differ from the above values by less than 0.5 kcal/mole. Comparison with the bridged structures shows that the top adsorption is more favored, especially for 0 2 9Larger binding energies for top structures means that, even for N2, the interaction energy with one Li cation includes a preponderant induction contribution (which is cancelled in the bridged geometries). Moreover, these results suggest that bridged geometries are probably not realistic structures for the N2 or 0 2 adsorption, except if the zeolite environment modifies differently the electrostatic and induction contributions.
114 3.3. I n t e r a c t i o n of N 2 and 02 with zeolite models 3.3.1 m ( L i +) a n d m ( N a +) Optimization of the structures of m(Li +) and m(Na +) clusters has led both Li + and Na + to form two equivalent XO bonds. The cation-(zeolite)O interaction is stronger in m(Li +) than in m(Na+), since the Li-O distance (1.88 A) is shorter than the Na-O distance (2.18 A). The potential energy curves (not corrected for BSSE) for the m(X+)Y2 clusters are depicted in Figure 5. These curves show that the binding energies for N2 are larger than those for 02 and that Li+-Y2 is still preferred to Na+-Y2, just as was found for q+-Y2 and X+-Y2 models. The binding energies corrected for BSSE indicate the same trend (3.7, 1.2, 2.6 and 0.9 kcal/mole for the Li+N2, Li+O2, Na+N2 and Na+O2 systems, respectively). Comparison with X+Y2 models shows that adsorption energies are smaller in the presence of the zeolite cluster but display the same relative ordering. The decrease of the calculated binding energies has to be related to the decreased positive charge attributed to the X cations, which is a consequence of charge transfer interactions between the aluminosilicate skeleton and its counterions. The net Mulliken charges are 0.79 for m(Li+)Y2 and 0.86 for m(Na+)Y2 , instead of a value of 0.95 for both Li+Y2 and Na+Y2 . These results indicate that the N 2 or 0 2 adsorption is, to first order, controlled by the Y2-cation interaction, whereas the zeolite framework plays a perturbative role, which can however modify the adsorption strength of these molecules.
0
-2
-2
E _~-4
E ---4
0
0
o
o .ar
v
v
LIJ
UJ
-6
-6 o -8
I
b I
a
v
c
e
b
v
d
v d I
2,5 3 3,5 r(X-Y) (angs) Figure 5. Potential energy curves of m(Li+)N2 (a), m(Li+)O2 (b),
m(Na+)N2 (c) and
o
m(Na+)O2 (d).
-8
I
2,5
I
I
3 3,5 r(Li-Y) (angs)
Figure 6. Potential energy curves of embedded Li+O2 a (site II), b (site [II) and Li+N2 c (site II), d (site III).
115
3.3.2 E m b e d d e d Li + and Na + m o d e l s The role of the small pentameric model of zeolite in N 2 or 02 adsorption can be depicted as a screening of the binding interaction with respect to free cations. This picture is however incomplete due to the small size of the cluster. Indeed, the long-range interactions between N 2 or 02 and the charge distribution of the zeolite framework are not negligible, since we have seen above that the electrostatic contributions decrease as 1/R 3. In order to take them into account in a further more realistic study, we have thus investigated how the previous X+Y2 descriptions are modified when they are placed in a representation where all surrounding atoms are replaced by appropriate point charges. Moreover, another purpose for this study was to delineate if this environment could modify specifically the adsorption properties of some cationic sites, with respect to N 2 or 02 molecules. In a very simple first attempt, conventional charges used in Molecular Mechanics simulations have been used for the zeolite atoms (values indicated in 3.2). Li cations have thus been placed at the coordinates of two neighboring cationic sites identified in faujasite as site II and site III, accessible to incoming gaseous molecules. These sites, located in a supercage, have been approached by N 2 or 02 molecules following a direction of lowest energy, roughly perpendicular to the zeolite framework around the cation, i.e. one six-membered ring for site II and two four-membered rings for site III. The binding energy curves for N 2 and 02 as a function of their distances from the Li cations in site II and site III are shown in Figure 6 (no BSSE corrections). The four curves have a minimum at around 2.3 A, which is longer than the equilibrium distances found for isolated cations and slightly shorter than the Li-Y distances evaluated for the m(Li+)Y2 models. The presence of the point charge network does not change the trend that N 2 is more strongly bonded to the cation than 02. Moreover, the binding energy difference between these two molecules, evaluated at 3.2 (site II) or 3.5 kcal/mole (site III) is similar to the value obtained from the pentameric model clusters (3.2 kcal/mole without BSSE correction). This difference was calculated at 4.4 for an isolated Li cation. If the presence of the point charge environment does not modify the relative ordering of N 2 and 02 adsorption energies, it clearly induces a difference between the adsorption property of cations in site II and site III. Indeed, the energy curves on Figure 6 show that site III is more favorable for adsorption than site II. Further calculations including larger clusters as well as more investigations on possible point charge sets are needed to confirm these preliminary results. 4. CONCLUSIONS These quantum mechanical calculations on small model clusters inluding Li and Na cations have shown that the different N2 and 0 2 adsorption properties in zeolites can be explained by simple arguments. Indeed, they have demonstrated
116 that a classical description involving electrostatic and induction energies, which depend on the quadrupole moment and dipole polarisability of these molecules repectively, is adequate to explain the basic reason for a stronger N2 adsorption. Moreover, the calculations show that a small cation like Li + behaves as a better attractor than a larger cation like Na +, the presence of the core electrons being the factor which limits the stabilizing contribution of the electrostatic and induction terms in the interaction energy. This conclusion justifies thus the use of classical simulations based on energy expressions including Lennard-Jones terms and also electrostatic (quadrupole) and induction contributions. The study of models including the zeolite as a cluster of atoms or as a network of point charges has shown that the zeolite framework has a perturbative role, screening the binding of both N2 and 0 2 , while leaving the main trends valid. A proper point charge embedding may help to rationalize the influence of the structure of the zeolite on the adsorption properties of specific sites.
REFERENCES
1. D.W. Breck, Zeolite Molecular Sieves, R.E. Krieger Publishing Company, Malabar (1984). 2. V.N. Choudary, R.V. Jasra, T.S.G. Bhat, Ind. Eng. Chem. Res., 32 (1993) 548. 3. C.G. Coe, J.F. Kirner, R. Pierantozzi, T.R. White, U.S. Patent No 5 152 813 (1992) and references therein. 4. D.H. Olson, J. Phys. Chem., 74 (1970) 2758. 5. I. P~pai, A. Goursot, F. Fajula, J. Weber, J. Phys. Chem., 98 (1994) 4654. 6. D.R. Salahub, R. Fournier, P. Mlynarski, I. P~ipai, A. St-Amant, J. Ushio, Density Functional Methods in Chemistry, J. Labanowski, J. Andzelm Eds., Springer-Verlag, New York, (1991) 77. 7. H. Sambe, R.H. Felton, J. Chem. Phys., 62 (1975) 1122. 8. B.I. Dunlap, J.W.D. Conolly, J.R. Sabin, J. Chem. Phys., 71 (1979) 3396. 9. A. St-Amant, D.R. Salahub, Chem. Phys. Lett., 169 (1990) 387. 10. A. St-Amant, Ph.D. Thesis, Universit~ de Montr6al, (1991). 11. C. Daul, A. Goursot, D.R. Salahub, Numerical Grid Methods and Their Application to Schrodinger's Equation, Cerjan, C., Ed.; NATO ASI Series, Kluwer Academic Press, 412 (1993) 153. 12. A.D. Becke, Phys. Rev. A, 38 (1988) 3098. 13. J.P. Perdew, Phys. Rev. B, 33 (1986) 8822; erratum in Phys. Rev. B, 38 (1986) 7406. 14. S.H. Vosko, L. Wilk, M. Nusair, Can. J. Phys., 58 (1980) 1200. 15. I. Phpai, A. Goursot, F. Fajula, D. Plee, J. Weber, J. Phys. Chem. to be published. 16. A.D. Buckingham, Intermolecular Interactions: From Diatomics to Biopolymers, Pullman, B.; Ed.; John Wiley & Sons, Chichester, (1978). 17. F. Visser, P.E.S. Wormer, W.P.J.H. Jacobs, J. Chem. Phys., 82 (1985) 3753.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
117
L o a d i n g and l o c a t i o n of w a t e r m o l e c u l e s in the zeolite clinoptilolite Y.M. Channon a, C.R.A. Catlow a, R.A. Jackson b and S.L. Owens c. aDavy Faraday Research Laboratory, The Royal Institution of Great Britain, 21 Albemarle Street, London, W 1X 4BS. bDepartment of Chemistry, Keele University, Keele, Staffordshire ST5 5BG. cCompany Research Laboratory, British Nuclear Fuels P.L.C., Springfields Works, Salwick, Preston PR4 0XJ. 1. INTRODUCTION This study concerns the application of computer modelling techniques to the behaviour of water in the zeolite, clinoptilolite. Such techniques have been extensively applied to dehydrated zeolites [1]; but their application to hydrated systems has been limited. Clinoptilolite is a naturally occurring zeolite that is a member of the heulandite group of zeolites. It has a unit cell formula NaxCayAl(x+2y)Si36_(x+2y)O72.24H20, and is isostructural with heulandite having an Si/A1 ratio of approximately 4. Clinoptilolite has a 2-D microporous channel system which was first characterised for heulandite [2]. Two channels run parallel to each other and the c-axis: channel A, a 10-member ring and channel B, an 8member ring. Another 8-member ring, channel C, lies along the a-axis and intersects the A and B channels. Figure 1 clearly shows channel A and B.
Figure 1 Structure of clinoptilolite showing the channels A, the 10 - member ring and B, the 8-member ring.
118 Widely used in industry and employed in gas separation and ion exchange [3], the material has a strong affinity for aqueous caesium and strontium ions, even in the presence of other aqueous cations [4, 5]. This property is exploited via ion exchange in the nuclear industry, and clinoptilolite was used to decontaminate the surrounding area after the accidents at Chernobyl and Three Mile Island [6]. Investigation of the loading and location of water in the zeolite is of importance owing to the influence water molecules exert on the structural and chemical properties by binding certain extra framework cations at specific positions within the framework. Although the location of water and the strength with which it is bound to the structure have been studied experimentally [7, 8], the location of cations and water molecules, as well as the coordination of these species within the structure is still poorly understood. As noted there have been many computational studies on dehydrated zeolites [9, 10], but few on hydrated systems. In this paper we report the first attempts to model hydrated clinoptilolite, and focus on the networks of hydrogen bonded water molecules that form inside the siliceous and aluminium substituted material. 2. M E T H O D O L O G Y Our work is based on the use of 'force field' methods, i.e. techniques employing interatomic potentials. The models used for the latter are described before we summarise the main techniques involved in the study.
2.1 Interatomic Forces Interatomic potentials describe the total energy as a function of the nuclear co-ordinates. These potential functions can be analytic or numerical. There are two broad categories of potential models; first those based on the Born and other related models for ionic solids which describe the system in terms of ions interacting via short and long range terms. The second type is molecular mechanics forcefields; these describe explicitly the bond angles and torsions for each specific system with the energy being given as a function of bond angles, lengths, torsional planes and other cross terms and their associated deviations from equilibrium values. The present study uses the molecular mechanics forcefield cff91_czeo (distributed by BIOSYM Technologies [ 12]), which has been specifically designed to be used in zeolite simulations. This forcefield is used with the following simulation techniques. 2.2 Molecular Dynamics This technique iteratively solves Newton's classical equations of motion. As discussed by Allen and Tildesley [ 13] a standard Taylor series is used to update positions and velocities by a suitable algorithm such as those first described by Verlet [ 13, 14]. The integration time step At, is typically 10-15 seconds. After the solution of the Taylor series equation, the original co-ordinates are replaced by the new ones, the velocities are updated and the acceleration is corrected by calculating the gradients, with the new co-ordinates. The work carried out in this study used the DISCOVER code [ 12] which embodies the Verlet algorithm.
119
2.3 Monte Carlo Techniques These generate ensembles by searching the configurational space of a system by a series of random moves, following for example, methodology developed by Metropolis and Ulam [15]. In the present case a simpler approach is used in which molecules are inserted randomly into the zeolite, and configurations are accepted when their energies fall below a specified threshold. 2.4 Energy Minimisation This technique explores the potential energy surface to locate configurations of minimum energy, and as such yields only static information. Iterative numerical procedures are used to search for the minimum, employing both first and second derivatives of the energy function. The present study uses the code DISCOVER [ 12]. 2.5 Multi Docker Our aim is to locate low energy sites of sorbed water molecules in clinoptilolite. To achieve this the computational techniques use a combination of molecular dynamics, Monte Carlo and energy minimisation methods, all employing a molecular mechanics forcefield. Specifically we use the Docker code developed by BIOSYM Technologies [12] which employs the methodology described by Freeman et al [ 16]. A molecular dynamics simulation is carried out at 298K on a water molecule. This generates a library of possible conformers. A Monte Carlo algorithm is then employed to choose Table 1 Adsorption energy of water, for the lowest energy configuration, as a function of molecule number in system 1. Water Molecule Number Energy (kcal / mole) 1 -5.4 2 -11.4 3 -11.7 4 -5.5 5 -11.2 6 -11.5 7 -17.5 8 -12.3 9 -17.1 10 -12.2 11 -11.8 12 -12.3 13 -14.1 14 -12.5 15 -13.2 16 -12.1 17 -10.6 18 -12.5 19 -12.6 20 -10.3
120
randomly a conformation from the library and insert it at random within the zeolite framework. Each accepted configuration is subsequently energy minimised; the configuration with the lowest energy is then used as the starting structure and the process repeated until the zeolite contains the required number of sorbates. 3. R E S U L T S Our primary aim in the initial study was to identify the ways in which water molecules are accommodated within clinoptilolite and the nature of the resulting hydrogen bonding patterns. We present the results as applied to two systems.
3.1 System 1 Twenty water molecules of adsorption of water number and Table 1 lists molecules are adsorbed each other t
I
I
C~l
CO
.
.
~
were iteratively docked into this system. Figure 2 shows the energy (for the lowest energy configuration), as a function of molecule the adsorption energy for each water molecule. The first three water into the same channel B/channel C intersection, and interact with
I
I
I
t.ID
.
.
I
"4:)
.
.
I'~ .
r
I
I
I
O'.
.
I
I
I
(2:)
,-'-
Oq
cO
~
~
,"7"
,"7-
,"7-
~
I
I
I
I
I
143
',O
r',,,
co
O',
CD
~
'--
,"7"
~
"'-
C'q
-4 e o
E -6
-
-
,-
-
-,
.
.
.
.
,-
-
- , -
-
-~
-
-
7
-
-
J-
-
- ~ -
-
-,
-
-
7
-
-
,-
-
-,
-
-
-,
-
-
,-
-
- , -
-
-,
-
-
z
-
-
L_
ID ~
-8
,, -10
$I " -12
.
.
.
i i i i il i i i i ill i ill 'iiiiii' .
.
.
.
.
.
.
.
.
till
-14
-16 -18 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Water
Molecule
Number
Figure 2 Graph of adsorption energy for water molecules in system 1 and the framework via hydrogen bonds. The next three water molecules locate at the intersection of channel A and channel C, and interact with each other, and the framework but not with the first three (see figure 3). The addition of the seventh molecule joins the first six water molecules via a hydrogen bond, and the ninth water molecule locates in a position that creates a circular network of hydrogen bonded water molecules, figure 4. The location of the next ten water molecules is controlled by their interactions with the existing hydrogen bonded network. This is illustrated by figure 2, which shows very little variation in their relative adsorption energies. They all locate at positions near enough to the circular network to form small clusters with sorbates participating in the network as shown in figure 5.
121
Figure 3 Six water molecules in system 1
Figure 4 Large Circular Network of water molecules in system 1
Figure 5 Large network with small clusters of water molecules 3.2 System 2 Here we present preliminary results for a siliceous system containing an aluminium ion substituted for a silicon ion, with the framework charge balanced by an hydroxyl bridge oriented into channel B. Ten water molecules have been iteratively docked into this system. Figure 6 shows the minimum energy of adsorption of water as a function of molecule number, and table 2 lists the relative adsorption energy for each water molecule. The addition of the first seven water molecules takes place in the same intersection of channels B and C, forming linked clusters of hydrogen bonded water molecules that also interact with the framework via hydrogen bonds as illustrated by figure 7. At this point the channel intersection appears to be full and the location of the eighth water molecule is at the boundary of channel C. This is still close enough to interact with the large cluster via a hydrogen bond. The ninth and tenth water molecules adsorb into the adjacent C channel and begin to form a
122
0
"
t
2 -2
_.o 0
.
.
.
.
.
.
.
3 .
.
.
.
.
.
.
.
.
.
.
I
I
I
t
~,
5
6
7
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
I
8
.
.
.
.
.
.
9
.
.
.
.
.
.
.
]o .
.
-4
E i._
e
-6
. . . . .
'.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
.
o -~
-8
c
-10
tltl
-14
. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
Water Molecule Number
Figure 6 Graph of adsorption energy for water molecules in system 2 Table 2 Adsorption energy of water, for the lowest energy configuration, as a function of molecule number for system 2. water Molecule Number Energy (kcal / mole)
1
-5.6
2 -11.4 3 -10.7 4 -12.7 5 -10.5 6 -11.6 7 -13.5 8 -11.9 9 -11.4 10 -10.1 new cluster. They hydrogen bond to each other and the eighth sorbate, so creating a large network of hydrogen bonded small clusters as shown in figure 8. 4. DISCUSSION From figure 3 we can see how the first six water molecules have located, as two non interacting trimers in system 1. The adsorption energy of the fourth sorbate is almost the same as the first, reflecting a site similar to the first with no other water-water interaction. The adsorption energy of the seventh water molecule which links the two trimers has the minimum for this system. The low relative adsorption energy of the ninth water molecule also highlights the stability arising from linking the water molecules together through hydrogen bonded networks. At this point there is a large circular network of hydrogen bonded water molecules. Further addition of water molecules results in the formation of
123
Figure 7 Seven water molecules in system 2.
Figure 8 Ten water molecules in system 2.
small cyclic clusters interacting with each other via the large circular network. From these results it can be postulated that until the zeolite has been loaded with six water molecules, it is the confining effect of the structure that is the dominant influence; after this has been attained the dominant influence is the previous water structure, directing the next sorbate to form small trimer and tetramer clusters that are linked to each other via a large network of hydrogen bonds. Consider now system 2. Figure 6 has a totally different pattern from figure 2 and indeed until the addition of the sixth water molecule no distinguishable pattern of cluster formation is observed. The sixth water molecule locates at a position that forms a tetramer and trimer linked to each other by hydrogen bonds; but it is the seventh water molecule that has the lowest adsorption energy for this system. At this point two tetramers form, linked by a water molecule with hydrogen bonds forming a network of two clusters (see figure 7). The channel intersection is now full with water molecules, and the eighth water molecule must locate away from the intersection. It adsorbs at the boundary of channel C, and still along channel B, close enough to the large cluster to interact via a hydrogen bond. This water molecule acts as a link to a new cluster that begins to form on the addition of the ninth and tenth water molecules. From the results of system 1, it can be seen that when a new cluster begins to form there is a marked increase in the adsorption energy, although this increase does not occur if the initial cluster molecule is hydrogen bonded to another water molecule. Such is the case for the ninth molecule which begins a new cluster in the adjacent channel C, but is stabilised by the hydrogen bond to the eighth water molecule and thence the large cluster. The network of hydrogen bonds that has been built up for system 2 is quite different from that built up for system 1, which must be due to the influence of the aluminium and hydroxyl bridge. What both systems do have in common, however, is that the low adsorption energies
124 correspond to the formation of trimeric or tetrameric clusters. The system is even more stable if these small clusters can be linked together with hydrogen bonds to form large networks. The lack of interaction between water molecules and the hydroxyl bridge in system 2 is currently under investigation. It is thought that this may be due to the low loading of a small molecule into a structure containing channels of large dimensions, but it may of course, reflect inadequacies in the interatomic potentials. 5. CONCLUSIONS This study is only the first stage of developing an understanding of the behaviour of water molecules in clinoptilolite. The dominant influences in the location of each water molecule at low loading, and in zeolites in general, is the structure of the existing water network, although of course, the zeolite exerts an influence on the location of the sorbed molecule. These points are illustrated by the different hydrogen bonded water patterns built up, and the eight ring channels preferentially adsorbing water molecules over the ten ring channel. The formation of hydrogen bonded trimers and tetramers strongly influences the energy of the sorbed molecule. The linking of these small clusters also affects their stability. Future studies will be concerned with water behaviour at higher loadings, and different chemical potentials, using the Grand Canonical Monte Carlo methodology. Further studies of the interaction of water molecules with acid sites are also planned. 6. ACKNOWLEDGEMENTS We are grateful to British Nuclear Fuels p.l.c, for supporting this work. We are grateful to BIOSYM Technologies for supplying the Catalysis and Sorption software. 7. REFERENCES 1 C.R.A. Catlow (ed.), Modelling of structure and Reactivity in Zeolites, Academic Press, London, 1992. 2 A.B. Merkle and M. Slaughter, Am. Mineral. 53 (1968) 1120. 3 M.W. Ackley, R.F. Giese and R.T. Yang, Zeolites, 12 (1992) 780. 4 L.L. Ames, Jr. Am. Mineral., 45 (1960) 689. 5 L.L. Ames, Jr. Am. Mineral., 46 (1961) 1120. 6 L.J. King,, D.O. Campbell, E.D. Collins, J.B. Knauer and R.M. Wallice, in Proceedings of the 6th International Zeolite Conference, (eds. Olson, D. and Bisio, A.), Bt~tterworths, Guildford, (1984) 660. 7 K. Koyama and Y. Takeuchi, Z. Kristallogr., 145 (1977) 216. 8 R.L. Ward and H.L. McKague, J. Phys. Chem., 98 (1994) 1232. 9 C.J.J. den Ouden, R.A. Jackson, C.R.A. Catlow and M.F.M. Post, J. Phys. Chem., 94 (1990) 5286. 10 R.A. Jackson and C.R.A. Catlow, Mol. Sim., 1 (1988) 207. 11 M. Born and J.R. Oppenheimer, Ann. Physik., 84 (1927) 457. 12 BIOSYM Technologies Inc., 9685 Scranton Road, San Diego, CA 92121 U.S.A. 13 M.P. Allen and D.J. Tildesley, Computer Simulation of Liquids, Clarendon Press, Oxford, 1987. 14 L. Verlet, Phys. Rev., 159 (1967) 98. 15 N. Metropolis and S.J. Ulam, Am. Stat. Ass., 44 (1949) 335. 16 C.M. Freeman, C.R.A. Catlow, S. Brode and J.M. Thomas, Chem. Phys. Lett., 186 (1991) 23.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviotand S. Kaliaguine(editors) 9 1995 Elsevier Science B.V. All rights reserved.
125
Withdrawal of Electron Density by Cations from Framework Aluminum in Y Zeolite Deterlnined by A1 XAFS Spectroscopy D. C. Koningsberger a and J. T. Millerb "Laboratory of Inorganic Chemistry and Catalysis, Debye Institute, Utrecht University, P.O. Box 80083, 3508 TB Utrecht, The Netherlands bAmoco Research Center, 150 W. Warrenville Rd., Naperville, IL 60566-7011, USA
The local AI structure and charge density in Y zeolites have been determined by low energy, AI XAFS spectroscopy. The whiteline intensity indicates that the AI charge density in Y zeolites decreases with increasing charge of the exchanged cation and correlates with the acidity of the zeolite. This result is consistent with the model that polyvalent cations withdraw electron density from the hydroxyl groups increasing their acidity.
1. INTRODUCTION For most hydrocarbon reactions, alkali metal zeolites, for example Na-Y, are relatively unreactive. Exchange of alkali ions by polyvalent cations like Ca, or La results in increased acidity and catalytic activity. The catalytic activity increases with the increasing charge on the cation [1-3]. Early explanations for the enhancement in activity by cations exchanged into Y proposed that strong electrostatic fields are present within the pores of the zeolite. Because of the rigid structure of the zeolite, the charge on the cation is not fully compensated by the negative charge localized on the aluminum-oxide tetrahedra [4]. Polyvalent cations in low coordination sites were proposed as acid centers [5]. An alternative explanation suggested that cations generate acidic hydroxyl groups by hydrolysis of coordinated 1-120 [6,7]. The acidic hydroxyl groups were confirmed by infrared spectroscopy [8]. Exchange of the alkali ions by ammonium ions with subsequent calcination to produce H-Y generates Bronsted acid sites and enhanced catalytic activity compared to Na-Y. In the absence of non-framework AI, however, the catalytic activity of H-Y is low. The activity of H-Y is greatly enhanced by exchange of a small amount of La ions [9,10]. The polyvalent cations, present in the 13 cages [11], are thought to withdraw electron density from the hydroxyl groups increasing their acidity [9,10,12]. The acid strength and catalytic activity of the Bronsted sites are determined by the polarizing effect of the cation and increases with increasing charge of the cation. In the present study, the effect of the cation on the charge density of the A1 ion and the AI-O bond distance has been determined by AI XAFS spectroscopy. As the charge on the cation increases from Na to H to Ca to La, the electron density on the A1 decreases. The
126 charge on the Al ion parallels the acidity of the catalysts. By contrast, the A1-O bond distance is independent of the type of exchanged cation and was about 1.7 A.
2. EXPERIMENTAL Na-Y was a commercial zeolite (LZY-54) purchased from UOP. The sample crystallinity was confirmed by XRD and had a unit cell dimension of 24.676 A, ca. 56 A1/unit cell. The preparation of H-Y has previously been given [13]. Briefly, Na-Y was repeatedly ammonium exchanged and carefully calcined to give H-Y. The crystallinity by XRD was 98% based on Na-Y as a standard, and the unit cell dimension was 24.643/~, or 52 Al/unit cell (11.5 wt% Al and 0.13 wt% Na). H-CaY (and similarly H-LaY) were prepared by ion exchange of Na-Y three times by a ten fold excess of 0.5 M Ca(NO3)2. The Ca-Y was wash, dried at 100C overnight and calcined at 300C for 3h. The Ca-Y was ion exchanged three times with a ten fold excess of 2 M NH4NO3, washed, dried and calcined at 300C for 5 h. The elemental analysis for H-CaY was 11.6 wt% Al, 1.5 wt% Ca, and 0.2 wt% Na, and for H-LaY was 12.4 wt% Al, 12.4% La, and 0.4 wt% Na. Standard methods were used to determine the Si and Al NMR, and the number of acid sites were determined by NI-I3 TPD [14]. EXAFS measurements were performed at the sot~ X-ray XAFS station 3.4 of the SRS at Daresbury (UK). This station is equipped with a quatrz, double crystal monochromator, and harmonic contamination of the X-ray beam was minimized by collimating mirrors. The estimated resolution was 1.5 eV at the A1 K-edge (1559 eV). The data were collected simultaneously with a fluorescence and an electron yield detector. Datum was collected with a k-space scan mode (start, 3 sec.; end, 30 sec.), and six scans were averaged in order to minimize both high and low frequency noise. Sample preparation, reference compounds, experimental conditions and standard procedures for analysis of XAFS data have previously been reported [13]. The near edge spectra were determined from the electron yield data, and the fluorescence data were used to generate the EXAFS function. The data were analyzed using the latest version of the Utrecht University XAFS Data Analysis Program (XDAP) which allows for fitting in r-space.
3. RESULTS X-ray diffraction and N2 micropore volumes indicate that the four Y zeolites are highly crystalline. The Si NMR also indicate that there is little change in the Si/AI ratio of the H-Y H-CaY and H-La-Y compared with Na-Y. Although the ratio of the peak intensities of HLaY are unchanged, the resonances are significantly broadened. The Si/A1 ratio of all catalysts is about 2.5 [ 15]. The Al NMR of Na-Y indicate that all of the Al is in tetrahedral coordination. For H-Y, 85% of the Al are in tetrahedral coordination with about 15% in octahedral coordination. The Al NMR of H-CaY indicate that 85% of the A1 is in tetrahedral coordination with 10% in octahedral coordination. The remaining 5% A1 seems to be in a distorted tetrahedral coordination which appears as a shoulder (about 55 ppm) of the main tetrahedral resonance. For H-LaY, 55% of the Al is in a symmetric tetrahedral coordination,
127
i.e., a resonance at 60 ppm. Approximately, 10% of the A1 is octahedral, 0 ppm, while the remaining 35% of the AI occurs as a broad resonance centered at 30 ppm. Since the Si NMR indicate little loss of structural A1, this 30 ppm peak may be due to structural, tetrahedral AI located near La ions resulting in a distorted electronic coordination about the AI. For each AI in the lattice, charge balance requires one equivalent of univalent cation. The elemental composition of H-Y, H-CaY and H-LaY indicate that there are 4.2, 4.3 and 4.6 mmol/g of AI, respectively. In addition, the univalent cation charge (due to Na, Ca or La) for H-Y, H-CaY and H-LaY are 0.06, 0.8 and 2.8 mmol/g. The number of protons required for charge balance for each, therefore, is estimated to be 4.1.3.5 and 1.8 mmoVg. The number of acid sites which strongly chemisorb NH3 in H-Y, H-CaY and H-LaY were 3.9, 3.6, and 1.9 mmol/g, respectively, and is equivalent to the number of protons in each catalyst. In H-CaY and H-LaY the cations, Ca +2 and La +3, do not chemisorb ammonia and are not strongly acidic. The x-ray absorption near edge spectra (XANES) of Na-Y (solid line), H-Y (dotted line), H-CaY (dashed line), and H-LaY (dotted-dashed line) are given in Figure 1. There is a clear distinction in the white line of the four samples with the intensity increasing in the order Na-Y < H-Y < H-CaY < H-LaY. A
N3 E
it;
L_
0
J t'.
~ ",
i..' \~ "-, ~." \ ' ; : ,
e,-
~c-2
/h
O e~
'.- .... ",,.
I
L_
I
... .......
.
J
-- .2"--:,'"
0
,',1 L_ !
X 0
.__j 0
-5
I
1
I
1
0
5
10
15
20
Energy (eV) Figure 1. X-ray Absorption K-edge of AI (Normalized) for Na-Y (solid line), H-Y (dotted line), H-CaY (dashed line) and H-LaY (dot-dash line). Figure 2a and 2b show the average EXAFS spectum and the Fourier transform of Na-Y (solid line) and H-CaY (dotted line), respectively. The high signal-to-noise ratio of the EXAFS data allows for the detection of higher coordination shells. The node positions for the two catalysts are nearly identical and indicate little difference in the A1-O bond distance which is confirmed in the Fourier transform. The lower amplitude of the first shell AI-O peak in the Fourier transform of H-CaY indicates a larger distortion in the AI-O coordination in
128
comparison to that in Na-Y. Similarly, Figure 3a and 3b compare the EXAFS spectrum and Fourier transform for H-CaY (solid) and H-LaY (dotted). Again, the node positions of the two catalysts indicate little difference in the Al-O bond distance. The amplitude of the first shell A1-O peak of H-LaY is slightly lower than that of H-CaY indicating a slightly larger distortion of the A1-O coordination.
0.4
0.3
0.3
0.2
0.2 ~ , 0.1
~ 0.1 =,?. I--0
0
'c. -0.1
-0.1
u. -0.2
"0"22
3
4
5
6
7
8
9
"0"30
k (l/A)
1
2
3
4
R (A)
Figure 2. a) Raw EXAFS data, and b) Fourier transform (k 1 : Ak = 2.7-8.2 A"1) of Na-Y (solid line) and H-CaY (dotted line).
0.4
0.3
0.3
~E 0 2
a
0.2
b
ol
c.9 -0.1
-o.1 " 0 "2 2
,,~ -o 2
3
4
5
6
k (l/A)
7
8
9
-0 301 - ' - ' ~ ~ ~ ~ ~ ~
~
R (A)
Figure 3. a) Raw EXAFS data, and b) Fourier transform (k ~ 9Ak = 2.7-8.2 A "~) of H-CaY (solid line) and H-LaY (dotted line). The first shell A1-O peak in the Fourier transform of the zeolite samples were fit in rspace (both magnitude and imaginary parts) using a non-linear multiple shell fitting routine [13]. All catalytsts were fit over the same data range (k ~ weighted, AR = 0.5 - 2.0 A, Ak = 2.7- 8.3 A'~). The number of independent parameters (N~p = 2*Ak*AR/x + 1) was 6.3, and the
129 degrees of freedom (Nfrce = N,,ap - Nat) were 2.3. The first shell fit in r-space is given in Figure 4a for H-LaY. The data and the fit were inverse Fourier filtered over the same r-range and are compared in Figure 4b. The quality of the fits is typical for all catalysts. The coordination parameters are given in the Table. Systematic errors are minimized by using the same background subtraction and normalization procedures for all data sets and by calibration with the reference phase shift and back-scattering amplitudes. Although fitting in r-space increases the useful data range, at present, it is not possible to calculate the limits of accuracy. For all Y zeolites, the AI-O coordination number is 4 in agreement with tetrahedral coordination. In addition, the AI-O bond distance for all catalysts is similar, around 1.7 A, also consistent with an A1-O tetrahedral coordination. The disorder (DebyeWaller factor) in the A1-O coordination increases in the order Na-Y < H-CaY < H-LaY.
Table Coordination Parameters Parameters
N
Ac~2
R
AEo
(xl 0 3) (,~2)
(A)
(eV)
Coordination: AI-O
E
Na-Y
4.0
-0.004
1.70
1.4
H-CaY
3.9
-0.002
1.71
-0.5
H-LaY
4.1
0.000
1.70
-0.3
1
0.3
o02
I-.
A ~
0
0
"~ -0.1 -0 2
-0.3 ' 0
1
1
9
i
1
2 3 R (A)
4
-0 12
3
4
5
6
7
8
9
k (llA)
Figure 4. Results of fit in r-space (k 1 9Ak = 2.7-8.2 A "l', AR "- 0.5-2.0 A) for H-LaY (data: solid line, and fit: dotted line), a) Fourier transform, and b) Fourier filtered data from 4a.
130 4. DISCUSSION As shown in Figure 1 the white line intensity, representing a ls to 3p transition, is sensitive to the type of cation exchanged into the zeolite. The white line intensity is the highest for H-LaY and increases in the order Na-Y < H-Y < H-CaY < H-LaY. Previously it was shown for H-Y and Na-Y that the whiteline intensity was higher for H-Y than Na-Y [13]. For these catalysts, the order of the electron densities derived from the white line intensities is in agreement with theoretical calculations for zeolite clusters. For example, the positive charge on the A1 in a protonated aluminosilicate ring, H § A1SiO3(OH)6", is 1.52 while on a symmetrically coordinated Na-aluminosilicate ring, Na § AISiO3(OH)6, the AI charge is 1.43, or 0.09 electrons less on the protonated cluster [16]. The whiteline intensities in this study, therefore, indicate that the electron density on the A1 is lowest, or positive charge of the AI ion is highest, for H-LaY and increases in the order H-LaY < H-CaY < H-Y < Na-Y. Structural determination of the A1-O bond distance in H-LaY, H-CaY and Na-Y indicate that the average distance is very similar, 1.70, 1.71, and 1.70 A, respectively. Previously, the AI-O bond distance in Na-Y was reported as 1.62 A [13]. The longer distance reported here is due to better data quality and the different fitting procedure, i.e., fitting in r-space. The current fluorescence data show a more linear response with increasing energy allowing for more accurate background subtraction. In addition, for AI in zeolites, the maximum data range for EXAFS analysis is limited up to about 8.5 A~ due to the overlap of the Si K-edge. Fourier filtering for fitting in k-space, however, limits the useful data range to about 3.5 A l [ 13]. By fitting in r-space, the useful data range can be increased by about 2 A "l improving the accuracy of the Al-O bond distance determination. Applying this new procedure to the previous data obtained on Na-Y results in an A1-O bond distance of 1.68/~ in general agreement with the results from this study. Reanalysis of the previous EXAFS data of H-Y results in an AI-O distance of 1.67/~. The current results indicate that within the limits of accuracy the AI-O bond distance is not sensitive to the type of cation exchanged into the zeolite. The whiteline intensity indicates that the cation has a dominating effect on the electron density of the aluminum ions. The order of the electron density parallels the acidity of the catalysts. That is, the electron density of the aluminum ion is the lowest and the whiteline intensity is highest for the most highly acidic zeolite, e.g., H-LaY. Since the cations are coordinated to lattice oxygen ions, it is likely that the cations are withdrawing aluminum electron density through these coordinated oxide and hydroxide ions. The low electron density on the aluminum ion also suggests that the electron density of the lattice oxide ions is lower due to coordination with the cation. Since the acid sites in H-CaY and H-LaY are due to the protons, the correlation of the whiteline intensity with the acidity suggests that a higher acid strength in ion-exchanged Y is due to withdrawal of electron density from the hydroxyl groups by the nearby polyvalent cations consistent with the model for enhanced acidity proposed by Lunsford [9,10,12].
131 5. CONCLUSION Low energy A1 XAFS spectroscopy is a powerful technique for directly measuring the local AI-O bond distance and charge on the AI ion. The average AI-O bond distance determined by EXAFS spectroscopy is independent of the type of exchanged cation in zeolite Y. On the other hand, the whiteline line intensity is very sensitive to changes in the charge on the AI ions induced by exchanged cations and correlates with the catalyst's acidity. As the charge on the cation increases, the charge on the A1 decreases suggesting that polyvalent cations withdraw electron density from the AI through the oxygen ions. The correlation of the whiteline intensity with the acidity suggests that the origin of the enhanced acid strength is due to the withdrawal of electron density from acidic hydroxyl groups by the nearby polycation.
REFERENCES 1. R.C. Hansford and J.W. Ward, J.Catal., 13, (1966) 316. 2. P.E. Eberly Jr. and C.N. Kimberlin, Adv. Chem. Ser., 102, (1971) 374. 3. M.L. Poustma, Zeolite Chemistry and Catalysis, ACS Mono. 171, J.A. Rabo (ed.), ACS, Washinton, D.C., (1976) 437. 4. J.A. Rabo, P.E. Pickett, D.N. Stamires, and J.E. Boyle, Proc. 2nd Int. Cong. Catal., Editions Technip, Paris, II ( 1961) 2055. 5. P.E. Pickett, J.A. Rabo, E. Dempsey and V. Schomaker, Proc. 3rd Int. Cong. Catal., W.M.H. Sachtler, G.C.A Schuit and P. Zwietering, eds., North-Holland Publishing Co., Amsterdam, I (1965) 714. 6. C.S. Plank,, Proc. 3rd Int. Cong. Catal., W.M.H. Sachtler, G.C.A Schuit and P. Zwietering, eds., North-Holland Publishing Co., Amsterdam, I (1965) 727. 7. P.A. Jacobs, J.B. Uytterhoven, J. Chem. Soc., Faraday, 69, (1973) 373. 8. J.W. Ward, J. Catal., 10, (1968) 34. 9. J.H. Lunsford, Fluid Catalytic Cracking II, Concepts in Catalyst Design, ACS Sym. Ser. 452, M.L. Occelli (ed.), ACS, Washington D.C., (1991) 1. 10. R. Carvajal, P.-J. Chu and J.H. Lunsford, J. Catal., 125, (1990) 123. 11. A.K. Cheetham, M.M. Eddy and J. M. Thomas, J. Chem. Soc., Chem. Commun., (1984) 1337. 12. P.O. Fritz and J.H. Lunsford, J. Catal., 119, (1989) 85. 13. D.C. Koningsberger and J.T. Miller, Catal. Lett., 29, (1994) 77. 14. B.L. Meyers, T.H. Fleisch, G.J. Ray, J.T. Miller, and J.B. Hall, J. Catal., 110, (1988) 82. 15. Engelhardt, G.; Michel, D. High Resolution Solid-State NMR of Silicates and Zeolitesi John Wiley and Sons, 150 (1987). 16. R.A. van Santen, B.W.M. van Beest and A.J.M. de Man, Guidelines for Mastering the Properties &Molecular Sieves, D. Barthomeuf (ed.), Plenum Press, New York, (1990) 201.
This page intentionally left blank
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 1995 Elsevier Science B.V.
133
Geometry of the Active Sites m Zeolites under Working Conditions F. Fajula Laboratoire de Matrriaux Catalytiques et Catalyse en Chimie Organique, URA 418 CNRS, ENSCM, 8, rue de l'Ecole Normale, 34053 Montpellier Cedex, France I. INTRODUCTION Due to the large use of zeolitic materials in major acid-catalyzed industrial processes, the characterization and description of the acid sites, particularly BrOnsted-type acid sites, in zeolites has received continuous attention. Among heterogeneous catalysts, zeolites constitute a unique class of solids because the acid centres are crystallographycally well defined. BrOnsted sites in zeolites can be attributed to acidic protons covalently bound to one of the oxygens linked to lattice aluminium atoms for which they provide charge compensation. In principle, the position of the active catalytic sites in the tridimensional network as well as their local geometry in terms of bond angles, bond lengths and environment might be fully determined and their acid strength and reactivity predicted. Considerable progress in the understanding of zeolite acidity has been gained from extensive spectroscopic, quantum chemical and structure modeling studies (see [1-3] for recent reviews), However, the catalytic significance of theoretical considerations has been established definitely only in a limited number of cases. The reasons for such a situation are multiple. The real links between structural acid sites and actual active sites is not straightforward. Reactivity depends indeed on intrinsic acidity but also on the properties of the conjugate ion generated upon protonation and on the contribution of the zeolite framework oxygen atoms in the stabilization of intermediates and transition states. These factors are not always easy to delineate and take into account in calculations and model studies. On the other hand, there are several evidences that H-form zeolites with their full complement of charge compensating protons exhibit little, if any, activity for hydrocarbon conversion reactions such as cumene and hexane cracking [4-6]. Secondary treatments generating extra-framework phases definitely enhance activity by creating new catalytic centers [6-8]. Similarly, although Lewis sites are almost systematically detected on activated zeolites, their direct or indirect implication in the catalytic events remains a matter of debate [9-11 ] and little is known regarding their nature, strength and location. Another main limitation arises from the fact that the actual working surface of a zeolite may be deeply modified by the presence of adsorbed and chemisorbed species, not
134 necessarily participating directly to the catalytic process. These species may behave as spectators, being chemisorbed on other sites, act as poisons or introduce additional diffusion limitations. In the last decade great efforts have been dedicated to adapt conventional spectroscopic techniques, among which infrared and NMR spectroscopy being the most popular, for studying catalytic reactions under conditions that recreate, or at least mimic, actual working conditions. The merits of this approach for the description of the reaction mechanisms at the molecular level and the detection of unrevealed reaction intermediates are well established and have been widely reviewed [12-14]. The in situ protocol should prove also well suited for the identification of the active sites and monitoring the changes of their local geometry during catalytic reactions or acidity measurements. It is my aim, at this symposium devoted to the <
>, to consider briefly some recent examples of such studies and to stimulate discussion about them. The aspects concerning the fate of the bridging structural A1 -OH-Si groups being largely documented, they will not be considered here. The examples I choose deal with the direct spectroscopic observation of peculiar behaviours of zeolites in the presence of sorbates, such as the change in the coordination of aluminium in protonic zeolite Beta, the generation of very strong Lewis acidity on ZSM-5 upon adsorption of olefins and the manifestation of the synergistic effect betwen Bronsted and Lewis sites in Faujasite and Mazzite. 2. REVERSIBLE CHANGE OF THE COORDINATION OF ALUMINIUM Changes in the environment of silicon and aluminium atoms upon hydration-dehydration or adsorption of bases have been evidenced several times for aluminophosphates and silicoaluminophosphates [ 15-18]. The easy adjustment of the lattice in the presence of adsorbates favors the attack of the AIO4 tetrahedra by the bases and generates penta and hexacoordinated framework aluminium species. Such a mechanism is supposed to be at the origin of the Lewisaciditj in these materials [ 19]. A reversible AI'V/AIv' transformation in aluminosilicate zeolites has been suggested to occur in the protonic form of zeolite Beta [20]. 27A1 NMR studies of hydrated H-BEA revealed that 20% approximately of the aluminium atoms were octahedrally coordinated. Replacement of the protons by ammonium ions, by treatment of the zeolite with gaseous ammonia at 100~ or by sodium and/or pgtassium cations, by standard exchange procedures, led to the disappearance of the AlW NMR signal and to an increase of the intensity of the AIIv one (Fig. 1). Material balances demonstrated that no aluminium was extracted from the solid during these treatments. Density functional calculations performed on pentameric cluster models of zeolite Beta with optimized geometry [21] showed that, due to the strong electron affinity of protons, the structure of the AIO4 units was considerably distorted with Si-O and AI-O bonds of the Si-OH-AI bridges elongated and weakened. Moreover the least stable site was found to be the one associated with two four-membered tings in the framework. On these bases, and by analogy with what has been reported for
135
d
L
_
ppm Figure 1.27A1 MAS NMR spectra of zeolite B e t a a) hydrated H-form, b) sample a saturated with ammonia, c) sample b acid-exchanged, d) sample c potassium exchanged [20].
Figure 2 . 2 7
ml MAS
NMR
spectra of zeolite H-Beta. Sealed ampules : a) hydrated sample, b) sample dehydrated at 300~ c) sample b with ethanol adsorbed, d) sample c after reaction at 200~ [24].
bl
d)
It
'
pp.~
136 VPI-5 [22], the AlXaNMR signal in protonic zeolite Beta was thus attributed to framework aluminium atoms linked to 4 lattice oxygens, the oxygen of a hydronium ion and the oxygen of a water molecule. The unique behaviour of zeolite Beta, and particularly the formation of hexacoordinated 27 framework aluminium, has been further investigated by AI MAS NMR by following the changes in the environment of the aluminium nuclei during the dehydration reaction of ethanol into ethylene and water. The reaction was carried out in 5 mm o.d. sealed capsules which were placed directly in an aluminium-free home-made NMR probehead that could spin the capsule at speeds up to 4 kHz [23,24]. NMR spectra were recorded for the parent hydrated zeolite in the protonic form, for the zeolite dehydrated at 300~ under vacuum, for the dehydrated zeolite equilibrated with 10 Torr of ethanol or pyridine and finally, after heating the zeolite sample loaded with ethanol for 30 min at 200~ Figure 2a shows the characteristic 27A1MAS NMR spectrum of hydrated zeolite Beta [20] with signals at 55 and 0 ppm due to tetracoordinated and hexacoordinated aluminium atoms, respectively. The removal of adsorbed water molecules causes a strong distortion of the electric field symmetry around aluminium. The increase of the quadrupolar coupling constants leads to a broadening of the signals which are no longer detected under our conditions (Fig. 2b). Adsorption of ethanol (or pyridine) induces a relaxation of the structure (also evidenced by infrared spectroscopy) and allows to regain the resonance line of tetrahedral aluminium at 55 ppm (Fig. 2c) while that of octahedral aluminium is still not observed. The latter signal develops after ethanol had been dehydrated, producing nascent water molecules which coordinate distorted AIOaH units leading to a more stable octahedral environment (Fig. 2d). These observations are qualitatively consistent with our assignment of the O ppm line to framework hexacoordinated aluminium and confirm the role of adsorbed water in generating it. Additional work is needed to reinforce this hypothesis and provide more quantitative data. The formation of hexacoordinated aluminium has been also postulated in steam dealuminated mazzite after a complexation treatment with acetylacetone [25]. The above results imply some flexibility of the zeolite lattice [26] or, at least, the presence of crystallographic sites able to suffer major local distortions without loss of long range crystallinity. As regards implications for catalysis using Beta zeolite, the change in symmetry of some aluminic sites will certainly modify their chemical feature. This may be of little importance in the case of the conversion of hydrocarbons (at high temperatures and with a low surface coverage by water) but could become significant for reactions involving polar substrates in the presence of solvents. 3. GENERATION OF LEWIS ACIDITY BY ADSORPTION OF HYDROCARBONS Medin et al [27] were the first to report on infrared studies of adsorbed acetonitrile and ammonia on H-ZSM-5 showing that olefms pre-chemisorbed at room temperature generated strong Lewis sites which were not detected in the freshly pretreated zeolite. As illustrated in
137 Figure 3a, the infrared spectrum of CD3CN adsorbed on the clean surface in the frequency -1 range of CN vibrations reveals the sole presence, at 2295 cm , of molecules coordinated to acidic hydroxyl groups. In the presence of pre-chemisorbed propylene, a second -1 signal at 2370 cm develops (Fig. 3b) that the authors attributed to new Lewis sites strongly interacting with the base. The formation of the new sites was / completely reversible as they disappear / after desorption at 500~ and readsorption of base. A very similar 0~ effect was observed when using I ammonia as probe. This unusual l 2~70 manifestation of Lewis acidity has been (U I I t.~ 50 explained by the cleavage of AI-O ! b). bonds in bridged alkoxyl groups and I inversion of the AIO4 tetrahedra to which the base molecules coordinate T 2~5 (Fig. 4). Support to this hypothesis was provided by quantum-chemical 100 L I ', 1 2 2400 2~00 2200 21 O0 calculations showing that the process Wavenumbers depicted by figure 4 would be Figure 3. Infrared spectra of CD3CN adsorbed energetically unfavorable for R = H but on H-ZSM-5 ' a) fresly pretreated sample, would become possible when R is an b) sample containing pre-adsorbed propene [27]. alkyl group. Such an interpretation was disputed by Bystrov [28] who explained the above results by invoking the formation of nitrilium cations in which acetonitrile is complexed to carbenium ions, the latter acting as very strong Lewis sites. The hypothesis of Bystrov has been elegantly confirmed by Jolly et al [29] who investigated the surface acidity of ZSM-5 in the presence of a series of pre- (or co-) adsorbed olefins choosen so as to generate carbenium ions with different structures. As expected, different nitrilium complexes were obtained using methylcyclopentene (signal at 2376 cm , Fig. 5c, d) and cyclohexene (signal at 2385 cm , Fig. 6a), due to interaction of acetonitrile with tertiary and secondary carbenium ions, respectively. The method was also able to detect the two carbenium ions, cyclohexyl and methylcyclopentyl, involved in the cyclohexene isomerization reaction (Fig. 6b,c) as well as those involved in the rearrangement of adsorbed propene oligomers. Two main conclusions can be drawn from this study. Firstly, nitriles constitute very efficient probes for the identification of adsorbed carbenium ions which are the intermediates of most hydrocarbon acid-catalyzed reactions. Secondly, under working conditions, the acidity of the surface is significantly modified. The strong Bronsted acid sites of ZSM-5 do
138 R
I X
o / \ X
Si
/I
I
1.6
b s o
1.4;
;
/
/
\
o
-,
!
,o
0
/
/
0
X/ Si
/I
O O I \
I
\
O "o" / \
/~
~
2376
\
I ~ ~ ^
/~
l
X "AI...B
/7
OO
1
'.'---~
o
+ B,-
IX
\
A
I
0 AI
O O
Figure 4. Proposed mechanism for the generation of Lewis acidity according to Medin et al. [27].
R
d) c)
0.4
b)
0.2 0.0
4000
~
3500
~
3000 2500 Wavenumbers (cm-1)
"
a)
2000
Figure 5. Infrared spectra of methylcyclopentene adsorbed on H-ZSM-5 9 a) freshly pretreated sample, b) aider adsorption of CD3CN, c) immediately aider adsorption of methylcyclopentene, d)aRer 1 h [29]. 0.8 0.7-
2300
0.6-
c) b)
0.50.4-
a) 0.3. 0.2
2soo
24bo
-2~
22bo
2~00-
Wavenumbers (cm-1)
Figure 6. Isomerization of cyclohexene on ZSM-5. Infrared spectra of CD3CN adsorbed after a) 1 h at RT, b) 1 h at 50~ c) 5 min. at 200~ [29].
139 not exhibit sufficient strength to form nitrilium ions [29,30] whereas the intermediate carbenium ions they generate do. Moreover, not only the strength, but also the nature of the acidity is modified. Both factors should be considered when dealing with complex reactions such as, for example, coke formation or paraffin/olefin alkylation.
4. SYNERGY BETWEEN LEWIS AND BRONSTED SITES.
4.1. The 3600cm
-1
infrared signal in faujasites
Several infrared studies of steam dealuminated faujasite have pointed out the enhanced acid strength (they are able to protonate acetonitrile) of hydroxyl groups characterized by a -1 stretching vibration frequency of 3600 cm [5, 8, 11, 31 ]. They are supposed to correspond to OH groups pointing to the large cage, perturbed by cationic tetrahedral aluminium present as A1OH+ entities in the beta cages. This signal is not observed on faujasites dealuminated by isomorphous substitution, free from extra framework species. The higher efficiency of these sites for the conversion of hydrocarbons has been demonstrated by using an infrared cell as catalytic reactor, operated under dynamic conditions at a temperature of 400~ [6,1 l!i Activity for n-hexane cracking was definitely associated with the presence of the 3600 cm OH groups. Regular high frequency OH hydroxyls and Lewis sites were inactive. All the accessible OH groups were found, by contrast, active for the conversion of cyclohexene, a -1 less demanding reaction. A direct relationship betwen the intensity of the 3600 cm signal and n-hexane cracking activity did not exist however since poisoning experiments using 2,6-1 lutidine and pyridine revealed that the 3600 cm OH groups were heterogeneous, only some of them being acidic enough to initiate the reaction.
4.2. Formation of iminium ions on mazzite. A recent study of the surface acidity of dealuminated mazzite using infrared and ultraviolet spectroscopy of adsorbed pyridine provided a direct evidence for the presence of very strong acid sites associated with Br6nsted/Lewis pairs [32]. At very low coverages in base, infrared bands at 2914, -1 2848, 1496 and 1462 cm and an ultraviolet signal at 205 nm, Figure 7. Dihydropyridistinct from those attributable to A i ~ dinium ion formed pyridinium ions and coordinated Oby reaction of pyridine pyridine, were detected. These on a BrOnsted/Lewis spectral features were pair of sites [32]. characteristic of a conjugated system containing aliphatic CH 2 groups and have been thus assigned to iminium L (dihydropyridinium) ions (Fig. 7). Their formation results
140 from a nucleophilic attack and protonation of pyfidine molecules adsorbed on Lewis sites and requires, therefore, the presence of paired Lewis/BrOnsted sites. Since loss of the aromaticring resonate energy is an energetically demanding process we can expect that the sites on which iminium ions form exhibit a very strong acid character. Additional experiments using heat-flow calorimetry and X-ray photoelectron spectroscopy confirmed the presence of such very strong sites [33]. The formation of iminium ion is not specific to mazzite and does not require, apparently, a particular spatial arrangement of the acid sites. An infrared signal at 1462 cm-1 that could characterize adsorbed pyridinium species has also been observed after high-temperature desorption of pyridine on a series of zeolites with different structures [32], on amorphous silica-alumina [34] and on clays [35]. Proton mobility or migration of cationic species with strong Lewis character may thus also account for this phenomenon. NMR and modeling studies are underway to clarify this point. 5. CONCLUDING REMARK. Experimental approaches aiming at a description of the fate of the active sites of acidic zeolites in the presence of adsorbed reactants or probe molecules may provide a less conventional picture of the surface than the one traditionally emphasized through well established structural and physical aspects of zeolite chemistry. These experiments are certainly promising to refine our understanding of the interaction between reactants and products with the inorganic framework at a molecular scale. In the present state of the art, the information available in the literature is, however, rather limited and essentially qualitative. The technical difficulties associated with the characterization of actual catalysts under non-ideal spectroscopic environments constitute undoubtly, to day, a major limitation. Considerable progress can be nevertheless expected in the future on account of the extensive efforts dedicated to the design of spectroscopic probes simulating reactor conditions. REFERENCES 1 J. Sauer, Stud. Surf. Sci. Catal., 84 (1994) 2039. 2. R.A. van Santen, Stud. Surf. Sci. Catal., 85 (1994) 273. 3 V.B. Kazansky, Stud. Surf. Sci. Catal., 85 (1994) 251. 4. S.J. DeCanio, J.R. Sohn, P.O. Fritz and J.H. Lunsford, J. Catal., 101 (1986) 132. 5. R. Carvajal, P.J. Chu and J.H. Lunsford, J. Catal., 125 (1990) 123. 6. S. Jolly, J. Saussey, J.C. Lavalley, N. Zanier, E. Ben~zi and J.F. Joly, Ber. Bunsenges. Phys. Chem., 97 (1993) 313. 7. R.M. Lago, W.O. Haag, R.J. Mikovsky, D.H. Olson, S.D. Hellring, K.D. Schmitt and G.T. Kerr, Proceedings, 7th Intern. Zeolite Conf., Kodansha, Tokyo, p 677, 1986. 8. F. Lonyi and J.H. Lunsford, J. Catal., 136 (1992) 566. 9. Y. Hong, V. Gruver and J.J. Fripiat, J. Catal., 150 (1994) 421. 10. G.R. Bamwenda, Y.X. Zhao and B.W. Wojciechowski, J. Catal., 150 (1994) 243. 11. S. Jolly, J. Saussey and J.C. Lavalley, J. Mol. Catal., 86 (1994) 401.
141 12. J.A. Rabo and G.J. Gajda, Catal. Rev. Sci. Eng., 31 (1990) 385. 13. J.F. Haw, NMR Techniques in Catalysis, A.T. Bell and A. Pines, Eds., Dekker, New York, 1994, P 139. 14. I.I. Ivanova and E.G. Derouane, Stud. Surf. Sci. Catal., 85 (1994) 357. 15. L.M. Kustov, S.A. Zubkov, V.B. Kazansky and L.A. Bondar, Stud. Surf. Sci. Catal., 69 (1991) 303. 16. A. Stein, B. Wehrle and M. Jansen, Zeolites, 13 (1993) 291. 17. P.J. Grobet, J.A. Martens, I. Balakrishnan, M. Mertens and P.A. Jacobs, Appl. Catal., L21 (1989) 56. 18. R. Vomscheid, M. Briend, M.J. Peltre, P. Massiani, P.P. Man and D. Barthomeuf, J. Chem. Soc., Chem. Commun.,6 (1993) 544. 19. M. Derewinski, M. Briend, M.J. Peltre, P.P. Man and D. Barthomeuf, J. Phys. Chem., 97 (1993) 13730. 20. E. Bourgeat-Lami, P. Massiani, F. Di Renzo, P. Espiau, F. Fajula and T. Des Couri6res, Appl. Catal., 72 (1991) 139. 21. I. Papai, A. Goursot, F. Fajula and J. Weber, J. Phys. Chem., 98 (1994) 4654. 22. L.B. McCusker, Ch. Baerlocher, E. Jhan, and M. B01ow, Zeolites, 11 (1991) 308. 23. F. Rachdi, J. Reichenbach, L. Firlej, P. Bernier, M. Ribet, R. Aznar, G. Zimmer, M. Helme and M. Mehring, Solid State Commun., 87 (1993) 547. 24. W. Buckermann, L.C. De Menorval, F. Figueras and F. Fajula, J. Phys. Chem., Submitted. 25. W. Buckermann,B.H. Chiche, F. Fajula and C. Gueguen, Zeolites, 13 (1993) 448. 26. J.A. Rabo and G.J. Gajda, NATO ASI Ser. B, Physics, Vol. 221 (1990) 273. 27. A.S. Medin, V. Yu, V.B. Kazansky, A.G. Pelmentschikov and G.M. Zhidomirov, Zeolites, 10 (1990) 668. 28. D.S. Bystrov, Zeolites, 12 (1992) 328. 29. S. Jolly, J. Saussey and J.C. Lavalley, Catal. Let., 24 (1994) 141. 30. J.F.Haw, M.B. Hall, A.E. Alvaro-Swaisgood, E.J. Munson, Z. Lin, L.W. Beck and T. Howard, J. Amer. Chem. Soc., 116 (1994) 7308. 31. G. Garralon, A. Corma and V. Fornes, Zeolites, 9 (1989) 84. 32. B.H. Chiche, F. Fajula and E. Garrone, J. Catal., 146 (1994) 460. 33. D. McQueen, B.H. Chiche, F. Fajula, C. Guimon, A. Auroux, F. Fitoussi and Ph. Schulz, J. Catal., Submitted. 34. K.H. Bourne, F.R. Cannings and R.C. Pitkethly, J. Phys. Chem., 74 (1970) 2197. 35. S. Bodoardo, F. Figueras and E. Garrone, J. Catal., 147 (1994) 223.
This page intentionally left blank
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
143
Characterization of Hexagonal and Lamellar Mesoporous Silicas, Alumino- and Gallosilicates by Small-Angle X-Ray Scattering (SAXS) and Multinuclear Solid State N M R Zelimir Gabelica 1, Jean-Marc Clacens 1, Roger Sobry2 and Guy Van den Bossche 2 1Laboratoire de Catalyse, FacultEs Universitaires Notre-Dame de la Paix, 61 rue de Bruxelles, B-5000, Namur, Belgique 2Laboratoire de Physique Exp6rimentale, Universit6 de Liege, Institut de Physique, b~timent B-5, B-4000, Li/~ge, Belgique
SUMMARY
Various mesoporous silicas and the corresponding alumino- or gallosilicates have been synthesized using a series of literature or home made recipes. The efficiency of the A1 or Ga incorporation markedly depends on the trivalent source and the evolution (aging) of the so formed Si-M(III) gel-type phases at different starting pH values, prior to the addition of the surfactant-structuring compounds. Low temperature (e.g. < 100~ syntheses yielded mesoporous compounds with hexagonal topology (MCM-41 type), involving thin multilayered Si walls (29Si-NMR data), eventually partly substituted for by A1 or Ga, (27A1and 71Ga-NMR). Such structures do remain stable after calcination in air at 600~ (TG-DSC and sorption data). The calcination either results in the expulsion of the (too voluminous) Ga(III) ions from the framework, or to a structural rearrangement of the remaining A1 species. The resulting solids still exhibit quite strong Br6nsted type acidic sites (NH3-TPD data). When the same gels are crystallized at 150~ fro 2 days, lamellar frameworks (MCM50 type) are preferentially stabilized. They readily collapse upon heating but the final amorphous phase still involves both A1 and/or Ga cationic (acidic) species randomly distributed in various structural environments. Small-angle X-ray scattering (SAXS) proved to be the choice method to unambiguously identify different topologies. The actual roughness (smoothness) of the various as-synthesized or calcined phases could be directly related to the fractal dimension derived from SAXS spectra. The presence of peaks at very small diffraction angles allowed us to estimate that the channel lengths of the thermally stable mesoporous materials essentially extend in the 150-200 nm range. EXPERIMENTAL
The different synthesis procedures adopted in this study were either literature recipes [1-3], sometimes slightly or thoroughly changed by home performed modifications [4]. All
144 the as-synthesized and calcined phases were characterized by using a combination of conventional techniques: powder XRD (topology, purity), atomic absorption and/or EDX (extent of trivalent incorporation), 27A1-, 71Ga- and 29Si- high resolution solid state MAS NMR (coordination and structural quantitative repartition of Ga and A1 bearing species, as well as the various Qx configurations of the Si atoms), TG-DTA-DSC-DTG combined with in situ n-hexane sorption (thermal stability, template content, pore volume determination, crystallinity), BET (surface area) and NH3-TPD (acidity). SAXS data were collected with a Kratky camera (Cu Ks radiation) using an experimental setup specifically built in the Liege University physics department [5]. RESULTS AND DISCUSSION
Gels prepared according to recipes as described in the literature [2,3] and left to crystallize at high temperature (i.e. 150~ for at least 2 days, yield well crystalline mesoporous lamellar (L) type phases. They exhibit good crystallinity (XRD data, high template content), medium surface area (< 500 ma/g) but their lamellar structure collapses as soon as they are heated under conditions currently used to remove the templates from mesoporous materials (600~ air flow). Conversely, thermally stable phases exhibiting a hexagonal (H) topology and a high surface area (> 1000 m2/g) could be prepared by crystallizing the same gels under milder conditions (at temperatures < 100~ or by modifying the gel composition (addition of TMA and/or under a careful pH adjustment and control). In both H and L structures, the degree of A1 incorporation dramatically depends on the nature of the Si and A1 starting materials, their solubility and their final degree of (de)polymerization at the end of the aging process at controlled pH, prior to any template addition. For equivalent experimental conditions, gallium tends to incorporate the final Si framework more quantitatively than aluminum. However, when both trivalents are added simultaneously (as oxides in the presence of various solubilizing additives such as NH3), their degree of incorporation is equivalent (Table 1). In the as-synthesized products, Ga is only partly sited in tetrahedral positions in both the H and L structures, as ascertained by 71Ga-NMR [6]. However, part of it remains either as a dispersed amorphous phase intermixed with the mesoporous compound, or incorporated in its framework, but randomly partitioned throughout the less well defined coordination sites, at least not detectable by NMR. In contrast, all the AI(III) ions are found located in both tetrahedral (T) and octahedral (O) framework sites, in various proportions that could be quantified [4]. Their repartition was shown to strongly depend on the synthesis conditions. After template removal upon calcination, the aluminosilicate phases generally show a better thermal resistance than the corresponding Ga analogs, although a partial dealumination and a marked framework (O) and (T) A1 redistribution is observed by 27A1-NMR. When gallium bearing L type phases are calcined, some residual Ga sited in T positions is still detected by NMR. These phases involve both Q3 and Q4 silicon configurations in various proportions, as seen by 29Si NMR, thus suggesting that both terminal silanols and Si(4Si) structural entities are present. The relative amount of Q3 and Q4 configurations could be quantified, provided the appropriate repetition times between 2 NMR pulses are selected in each case (the Si nuclei in the as-synthesized and calcined phases do relax very differently
145 [4]. Assuming that Q3 essentially corresponds to the terminal hydroxylated surface while the Q4 configurations reflect the non defected bulky Si structure, the calculated Q3/Q4 ratios could be related to the actual thickness of the framework (essentially siliceous) walls. It could be concluded that the lattices of the L type phases involve at least 5 or more Si layers, in which Ga still can find a stable T coordination within the internal layer(s). Table 1A Synthesis conditions Code
Source of trivalent element
T(~
/ time
Synth. cond. [ref.] (1)
1/9 2/11
A1203 Na Aluminate
150 / 65 h 150 / 65 h
[3 a] [3 a]
3/12
---
150 / 65 h
[3 b]
4/14
Na Gallate
150 / 65 h
[3 a]
5/15 6/20
Ga203 Na Aluminate (NH 3)
150 / 65 h 150 / 65 h
[3 a] [3 c]
7/21
Ga203 (NH 3)
150 / 65 h
[3 c]
8/22
A1203 + Ga203 (NH 3)
150 / 65 h
[3 c]
15/7 9/17-1
A1203 (TMA) ---
150 / 65 h 150 / 65 h
[1,5] [4,5]
10/17-2
---
100 / 6 days
[4,5]
11/18-1
A1 Sulfate
150 / 65 h
[4,5]
12/18-2
A1 Sulfate
100 / 6 days
[4,5]
13/19-1
Ga Sulfate
150 / 65 h
[4,5]
14-19-2
Ga Sulfate
100 / 6 days
[4,5]
(1) Letters a, b and c refer to variants in the synthesis recipes described in reference [3]
146 Table 1B Some characteristics of the final mesoporous phases obtained by using various synthesis conditions Final product Code
Nature (1)
1/9 2/11
L L
% incorporation Si
A1
88 (nd) (2)
100 18
Si/M (at.) Ga 24 (nd)
3/12
L
87
---
4/14
L
100
---
81
5/15
L
100
---
84
6/20
L
(nd)
93
45 43 (nd)
7/21
L
100
---
94
26
8/22
L
100
80
76
20
15/7
H
100
41
9/17-1
L
(nd)
---
36
10/17-2
H
(nd)
---
11/18-1
L
100
16
12/18-2
H
88
100
13/19-1
L
(nd)
---
98
(nd)
14/19-2
H
87
---
96
90
311 44
(1) L: lamellar phase; H: hexagonal phase (2) (nd) not determined Similarly, all the as-synthesized H type phases also exhibit a quite broad NMR resonance that could be deconvoluted into two lines of variable intensity, one located a t - 100 ppm and better corresponding to Q3 configurations, the other a t - 110 ppm, assigned to Q4. It is actually not clear to which NMR line should be attributed the Si atoms being interacting with the bulky terminal -N(CH3) 3 groups of the CTABr templates and thus forming Si (3Si, IN) configurations, so that the estimation of the actual wall thickness from only the NMR data in the precursors is dubious, especially when the spectra are broad. After calcination, the spectra are better resolved and more Q3 configurations were detected, suggesting the presence of major silanol terminations in the final calcined hexagonal frameworks, in line with a Hoffman type degradation of the tetraalkyl ends of the template. An estimation of the Q3/Q4 ratios could be achieved. It still suggests the presence of multilayered walls of Si atoms, roughly composed of a maximum of 3-4 Si layers. Undoubtedly the walls of the H phases are thinner than those detected in the L type phases. Irrespectively to the smaller AI(III) ions, Ga(III) species are probably too bulky as to still
147 remain sited in the "peripheral" T positions of the hexagonal structure. Their expulsion is possibly more readily achieved because of the presence of important strains within the thin layers. Finally, the SAXS spectra of the various as-synthesized and calcined compounds strongly confirm the above detected structural features and, in most cases, bring more detailed structural characteristics about the thickness of the walls, the fractal slope, the smoothness of the external envelope and the length of the hexagonal channel systems. The presence of peaks at very small diffraction angles allowed us to evaluate the channel lengths of the thermally stable hexagonal mesoporous materials. Depending on experimental condition and on the presence of trivalent ions in the framework, the mean length essentially extends in the 150-200 nm range. The detailed SAXS study is discussed elsewhere [5]. REFERENCES
1. S.J. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonovicz, C.T. Kresge, K.D. Schmitt, C.T.W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCuller, J.B. Higgins and J.L. Schlenker, J. Amer. Chem. Soc., 114 (1992) 10834. 2. C.Y. Chen, H.X. Li and M.E. Davis, Microporous Materials, 2 (1993) 17. 3. K.M. Reddy, L. Moudrakovski and A. Sayari, J. Chem. Soc. Chem. Commun. (1994) 1059. 4. J.M. Clacens and Z. Gabelica, in preparation. 5. R. Sobry, G. Van den Bossche, J.M. Clacens and Z. Gabelica, in preparation. 6. Z. Gabelica, C. Mayenez, R. Monque, R. Galiasso and G. Giannetto, in: Synthesis of Microporous Materials: Vol. I: "Molecular Sieves" (M.L. Occelli and H. Robson, Eds.), Van Nostrand Reinhold, New York, 1992, 289.
This page intentionally left blank
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
149
CHARACTERISATION OF A CUBIC MESOPOROUS MCM-48 COMPARED TO A HEXAGONAL MCM-41 Raft Schmidta, b , Michael St6cker a and Ole Henrik Ellestada, b a SINTEF, P.O. Box 124 Blindem, N-0314 Oslo, Norway. b University of Oslo, Department of Chemistry, P.O. Box 1033 Blindem, N-0315 Oslo, Norway.
ABSTRACT A cubic MCM-48 and a hexagonal MCM-41 material were synthesised. The pore ordering was confirmed by X-ray powder diffraction and HREM studies. The pore size of the materials was determined to 2.9 nm for MCM-41 and 2.5 nm for MCM-48 by N 2 adsorption and by measuring the freezing depression of water enclosed in the pores by 1H NMR. The self diffusion coefficient of water confined in the pores of MCM-48, determined by 1H NMR spinecho measurements, was found to be significantly lar~er compared to that of MCM-41.29Si MAS NMR showed a significant higher number of Q J species (Si(3OSi)OH) for MCM-48 in the as-synthesised state compared to MCM-41. INTRODUCTION The discovery of a new family of mesoporous materials, denoted as M41S, was recently reported by researchers from the Mobil Oil Co-operation [ 1,2] and has dramatically expanded the range of defined pore sizes ( < 1.3nm) found in crystalline microporous materials (e.g. zeolites) into the mesopore regime ( > 2 nm). High hydrocarbon sorption capacity and high thermal stability are additional interesting properties of these materials. They are synthesised from gels, containing besides silica optionally different other metals (e.g. A1.). The structure of the porous solid is hereby defined by the aggregation of surfactant molecules (such as C16H33(CH3)3NBr) [1]. Already in the first publications [1,2] it was reported that purely siliceous materials with hexagonal ordered pores (MCM-41), layered materials (MCM50) and materials with a three dimensional pore system (MCM-48) could be synthesised by this mechanism, indicating the diversity of this new family of mesoporous materials. However, most of the academic interest following this new invention, was concentrated on MCM-41 [37] and only very few characterisation data of the cubic member of the M41S family (MCM48) have been published [5 - 7], even though the three dimensional pore system of MCM-48 may make this material even more interesting for industrial applications as MCM-41. Here we report on the synthesis of a MCM-48 and a MCM-41 material and the characterisation by
150 XRD, HREM, N 2 adsorption, 29Si MAS NMR and 1H NMR of water enclosed in the pores [8]. Additionally the self diffusion-coefficients of water enclosed in the pores of these mesoporous materials were determined by 1H NMR spin-echo measurements. EXPERIMENTAL A purely siliceous MCM-48 material was synthesised according to the following procedure (similar to the one described by Monnier et al. [5]): 0.7 g of NaOH was dissolved in 17 g of distilled water. Then 7.22 g of tetraethylortosilicate (TEOS) (98%, Jansen) was added to the gel while stirring. After 5 min 27.8 g of the template solution containing 25 wt% C16H33(CH3)3NC1 in distilled water (Fluka) was added. The molar composition of the gel was 1:0.65:62, respectively for TEOS : C16H33(CH3)3NC1 :H20. The resulting gel was then stirred for another 15 min, loaded into a stoppered Teflon bottle and heated without stirring at 100~ for 72 hr. After cooling to room temperature, the resulting solid was recovered by filtration, extensively washed with distilled water, and dried in air at ambient temperature. The template was removed by calcination at 540 ~ for 1 hr in flowing nitrogen followed by 6 hrs in flowing air with flow rates of 100 ml/min, respectively. A siliceous MCM-41 material was synthesised according to a procedure given by Beck et al. using C16H33(CH3)3NBr as template[2] and processed according to procedure described above. The obtained solid materials were characterised by X-ray powder diffraction (Siemens D5000 diffractometer, CuKo~ radiation) and High Resolution Electron Microscopy using a JEOL 2000 FX instrument applying primary magnifications between 68 000X and 210 000X. The TEM samples were prepared by crushing the material in ethanol in an agate mortar and dropping this dispersal of finely grounded material onto a holey carbon film. This produced free sheets of the material suitable for TEM work. Tilting of the specimen for accurate crystal alignment was usually not necessary. N 2 isotherms were measured at 77 K with a Carlo Erba instrument using a conventional volumetric technique. The samples were outgased at 200~ for 1 hr. The mean pore size was calculated from the N 2 isotherm using the Kelvin equation correcting for the mulfilayer thickness. The water-saturated samples were studied by 1H NMR in the temperature range 273 to 183 K using a Varian VXR 300 S NMR spectrometer, operating at 300 MHz proton resonance frequency [8]. All measurements were performed with a 90 ~ pulse of 16 Its. Each spectrum was composed of 16 transients. The samples were temperature equilibrated for 5 min at each temperature before any measurements were performed. The spectra were accumulated applying a temperature cycling, i.e., heating and cooling of the sample. Further T 2 measurements of water enclosed in the pores were performed at 268 K using Carr-Purcell-Meiboom-Gill (CPMG) pulse sequence with varying "cbetween 16 and 400 Its. The self diffusion coefficient of pore water was extracted from the obtained T 2 data using a model proposed by LeDoussal et al. [11]. 29Si MAS NMR spectra were recorded on the same spectrometer, equipped with a Jakobsen high spinning speed MAS probe using 7 mm zirconia rotors. Frequency of 59.6 MHz, sweep width: 1400Hz, pulse width 8 Its (90 ~ degrees pulse: 8.3 ~ts), repetition time: 300 sec, acquisition time: 1 sec, number of scans: 1000, MAS spinning speed: 4.5 kHz. The lines were referenced to the low field signal of ZSM-5 at -109.6 ppm (as a secondary reference).
151
RESULTS AND DISCUSSION
Well ordered MCM-48 and MCM-41 materials, confn'rned by XRD (Figures 1 and 2) and HREM (Figures 3and 4) were prepared.
t
d-value~ hki [4.~] 100 2.3 2.0
,--,
5 c6
d-values 4.19 3.59 2.73 2.48 2.25 2.15 2.06 1.98 1.84 1.63 1.56 1.47
110 200
21o II
1:53~ .
300 220
>, "~ r-"~ t
~
0
2
4
6
8
hid
[nm]
10
Degrees 2-theta
0
2
4
211 220 321 400 420 332 422 431 521 611/532 541 444 543
6
8
10
D~j rees 2-theta
Figure 1. X-ray powder diffraction data of the as-synthesised MCM-41
Figure 2 X-ray powder diffraction data of the as-synthesised MCM-48.
Figure 3. HREM image of as-synthesised MCM-41 in the direction of the pores.
Figure 4. HREM image of as-synthesised MCM-48 with pores on the 110 plane.
152 The X-ray diffractogram of the as-synthesised MCM-48 could be indexed according to a cubic space group with Ia3d symmetry, and a unit cell size of 102 A, which is in agreement with our HREM investigations. A representative electron micrograph of MCM-48 viewed along the [ 110] axis is shown in Figure 4. The unit cell size of the hexagonal MCM-41 was determined to 46/~ (Figure 1) and the hexagonal pore organisation was confirmed by HREM (Figure 3).The pore structure of MCM-48 was generally observed over the whole sheet investigated by HREM, even though small variations e.g. of the pore wall thickness could be registered. These variations result in the displacement of one single pore at the time, and not in the disturbance of the whole local structure. For MCM-41 local variations often result in a disturbance of the (hexagonal) pore organisation over a significant larger area than for MCM48. However, the pore structure of both materials is found to be quite unaffected by the removal of the template by a calcination at 540 deg C. The BET surface area was determined to be 1100 m2/g. and 1080 m2/g. for the MCM-48 and MCM-41, respectively. In accordance with the N 2 isotherms recorded for MCM-41 (Figure 5), the N 2 isotherm of MCM-48 showed a sharp increase in the adsorbed volume of N 2 due to capillary condensation of N 2 in the pores of this material (Figure 5).
~41~ I--v m
E
[
.~400 Figure 5. Nitrogen isotherm at 77 K on MCM-41 and MCM-48. Filled symbols denote adsorption, open symbols denote desorption.
0
E __=200 0 > |
0i 0
i
I
I
I
I
0,2
0,4
0,6
0,8
1
P/Po However, even though both materials were synthesised using C 16H33(CH3)3N+ as template the sharp increase in the adsorbed volume of N 2 due to capillary condensation occurs at different relative pressures P/P0; reflecting different pore sizes of the MCM-41 and MCM-48
153 material. Using the relative pressure (at the inflection point of the capillary condensation) of P/P0 = 0.35 for MCM-41 and P/P0 = 0.26 for MCM-48 and using the Kelvin equation correcting for multilayer thickness, the mean pore sizes were calculated to be 2.9 nm and 2.5 nm for MCM-41 and MCM-48, respectively. The pores of the MCM-41 and MCM-48 material were further characterised by 1H NMR temperature studies of water enclosed in the pores. The 1H NMR spectra of confined pore water of MCM-48 vs. temperature (from 265 to 183 K) are illustrated in Figure 6 and show clearly a sharp intensity decrease with decreasing temperature due to the freezing of pore water.
i
d >,
0
rr" Z "1, ..i. w
280
260
240
i
!
|
220
200
180
Temperature [ K] Figure 6. 1H NMR spectra of water enclosed in the pores of MCM-48 as a function of temperature. A mathematical model [8] was fitted to the 1H NMR signal intensity vs. temperature of water enclosed in MCM-41 and MCM-48 (Figure 7, solid line). Using this model a transition temperature of 224 K reflecting the freezing of the pore water was determined for MCM-48. For the MCM-41 material a transition was observed at 225 K while cooling and 228 K while wanning up. This observed hysteresis in freezing/melting transition (which is not observed for the MCM-48) is due to the larger pore size of the MCM-41 compared to MCM-48 and not due to the destruction of the pores during the freezing/melting process [9]. The effect of the pore size on the occurrence of freezing/melting transition is discussed in detail in a recent publication [10]. Using the freezing point depression (determined by warming up the water saturated samples form 183 K to 273 K, while recording the 1H NMR signal) the pore sizes of MCM-41 and MCM-48 were calculated to 2.9 + 0.08 nm and 2.7 + 0.16 nm, respectively. It was assumed that the observed freezing point depression (AT = 237.15 K - transition temperature) is correlated to the pore size by AT =
K/ R p - tl
9with Kf = 49.5 + 0.19 K*nm-1
154
and tf = 0.35 + 0.036 nm [9]. The pore sizes determined by N 2 adsorption and 1H NMR method are found to be in good agreement.
"L
MCM-41
"'7, :3
t'-
MC 48
Figure 7. 1H NMR signal intensity of pore water confined in MCM-41 and MCM-48. Filled symbols denote heating, open symbols denote cooling of the sample.
%
r
rr"
-
N
Z
"1-
280
260
240
220
200
180
T~rature [ K] The water saturated MCM-41 and MCM-48 samples were further studied by measuring the apparent spin-spin relaxation (T22) of the confined pore water at 268 K. The temperature of 268 K was chosen to ensure that water not enclosed in the pores is frozen and though does not contribute to the measured spin-spin relaxation time. Of particular interest is the dependence of the apparent relaxation rate, 1/T22, on the inter pulse time 2z. This behaviour has been discussed in the literature [11] and arises because of the motional diffusion of the water molecules through the magnetic field gradient created by the susceptibility difference between the solid matrix and the pore water. The apparent relaxation rate (1/T22) extracted from the observed CPMG echo envelope is therefore not only dependent on the inherent spinspin relaxation time of the enclosed pore water (T2), but also strongly affected by the fluid molecules moving (characterised by the diffusion coefficient D) in the inhomogeneous magnetic field within the pore: 1/T22 = 1/3 * ?2DG2z2 + 1/T 2, with ~/ the nuclear magnetogyric ratio, D the self diffusion coefficient of the pore fluid, G the magnetic field gradient G, and the inter pulse spacing z. For a porous medium this equation has to be modified to take into account the motional restrictions imposed by the pore walls. Applying the model derived by LeDoussal et al. [ 11] the self diffusion coefficient of the pore water can
155 be extracted from the measurements of the apparent spin spin relaxation times as a function of x. This is explained in detail for MCM-41 materials in a recent work by Hansen et al. [ 12]. The self diffusion coefficient for water enclosed in the pores was found to be 4.53 + 0.27 10-9 cm2/s for MCM-41 and 2.21 + 0.06 10-8 cm2/s for MCM-48 whereas the self diffusion coefficient (D) of bulk water at 300 K is approximately 2.5 10-5 cm2/s. This demonstrates a strong reduction of the diffusion coefficient of pore water compared to bulk water. In a previous study of MCM-41 materials D was found to decrease with decreasing pore size [12]. However, in this study a significantly higher self diffusion coefficient of pore water was calculated for MCM-48 compared to MCM-41 even though MCM-41 posses larger pores. This suggests a larger mobility of pore water in the three dimensional pore system of MCM-48 compared to the uni-dimensional pore system of MCM-41. However, other effects on D, as e.g. different particle sizes, validity of the model for the calculation of D, etc. may influence the result. This will be a subject of future studies. Through 29Si MAS NMR a significant larger number of Q3 species (Si(3OSi)OH) represented by the peak at around -100 ppm compared to Q4 (Si(4OSi) species represented by the peak around -110 ppm was observed for MCM-48 than for MCM-41 in their as synthesised state (Figure 8). A Q3/Q4 ratio of around 0.45 and 1 was found for MCM-41 and MCM-48, respectively.
-110 -100~"~
41
~ I
I
-50
-70
I
I
~-48 I
I
-90 -110 -130 -150 ppm
Figure 8.29Si MAS NMR spectra of MCM-41 and MCM-48. Resonances are assigned as follows" around - 100 ppm: Q3 _ species; around- 110 ppm" Q4_ species.
156 CONCLUSION Well ordered MCM-48 and MCM-41 were synthesised. The overall pore organisation of MCM-48 is much less affected by local variations (e.g. wall thickness) as for MCM-41. The pore size of the template free MCM-41 was found to be larger (around 2.9 nm) compared to MCM-48 (around 2.5 nm) synthesised with the same cationic template ( C 16H33(CH3)3N+)A good agreement between the determination of the pore size by N 2 adsorption and ~H NMR temperature studies of "pore water" was found. The self diffusion coefficient of water confined in the pores of MCM-48, determined by 1H NMR spin-echo measurements, was found to be significantly larger compared to that of MCM-41. A significant higher number of Q3 species (Si(3OSi)OH) was found for MCM-48 compared to MCM-41 in their assynthesised state. ACKNOWLEDGEMENTS A research grant from the Norwegian Research Council (Deminex program) is gratefully acknowledged by R.S.. The authors are indebted to E.H. TCrstad and A.Olsen for preparing the HREM micrographs and E. Hansen for recording the 1H NMR spectra and D. Akporiaye for fruitful discussions. REFERENCES 1. C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli, J.S.Beck, Nature 359 (1992) 710. 2. J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T-U. Chu, D.H. Olsen, E.W. Sheppard, S.B. McCullen, J.B. Higgins, J.L. Schlenker, J.Am. Chem. Soc., 114 (1992) 10834. 3. C.Y. Chen, H.X. Li and M.E. Davis, Microporous Materials 2 (1993) 17. 4. R. Schmidt, D. Akporiaye, M. St/Scker and O.H. Ellestad, J. Chem. Soc., Chem. Commun.(1994) 1493. 5. A. Monnier, F. Schiith, Q. Huo, D. Kumar, D. Margolese, R.S. Maxwell, G.D. Stucky, M. Krishnamurty, P.;Petroff, A. Firouzi, M. Janicke and B.F. Chemelka, Science 261 (1993) 1299. 6. J.C. Vartuli, K.D. Schmitt, C.T. Kresge, W.J. Roth, M.E. Leonowicz, S.B. McCullen, S.D. Hellring, J.S. Beck, J.L. Schlenker, D.H. Olsen and E.W. Sheppard, Chem. Mater. 6 (1994) 2317. 7. Q. Huo, D.I. Margolese, U. Ciesla, P. Feng, T.E. Gier, P. Sieger, R. Leon, P.M. Petroff, F. Schiith and G.D. Stucky, Nature 368 (1994) 317. 8. D. Akporiaye, E.W.Hansen, R. Schmidt and M. St/Scker. J. Phys. Chem., 98 (1994) 1926. 9. R. Schmidt, E.W. Hansen, M. St/Scker, D. Akporiaye and O.H. Ellestad, J. Am. Chem. Soc. in press. 10. R. Schmidt, M. St6cker, E.W. Hansen, D. Akporiaye and O.H. Ellestad, Microporous Materials 3 (1995) 443. 11. P. LeDoussal and P.N. Sen, Phys.Rev.B. 46 (1992) 3465 12. E.W. Hansen, R. Schmidt, M. St6cker and D. Akporiaye, Microporous Materials, submitted.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
157
Synthesis and Characterization of Transition Metal Containing Mesoporous Silicas S. Gontier and A. Tuel Institut de Recherches sur la Catalyse. C.N.R.S. 2, av. A. Einstein 69626 Villeurbanne Cedex France Titanium and Vanadium mesoporous silicas (MS) have been synthesized at ambient temperature using a neutral templating route with primary alkyl amines as surfactant. Spectroscopic characterization of the samples showed that transition metal cations were highly dispersed in the silica framework. The metal content, the surfactant chain length and the amine/SiO 2 ratio greatly influenced the properties of the final product. These materials were found to be active as catalysts in oxidation reactions with alkyl peroxides at mild temperature. 1. I N T R O D U C T I O N There has been an extensive interest during the last years for the synthesis of transition metal containing molecular sieves, due to their remarkable properties as catalysts in oxidation reactions with organic peroxides [1,2]. A very beautiful example is TS-1, the titanium substituted silicalite-1, that catalyzes many oxidation reactions in the liquid phase with aqueous hydrogen peroxide. However, as far as zeolitic supports are concerned, reactions are limited to small substrates with a kinetic diameter smaller than 7~. Recently, the discovery of a novel family of silica-based mesoporous molecular sieves M41S by Mobil researchers [3] and a group from Waseda University [4] opens new perspectives in the field. Corma et al. [5]
were the first to synthesize a Ti
mesoporous silica analog to MCM-41 and to show that the material was active as catalyst in the oxidation of bulky substrates. In a similar manner, Franke et al. [6] also prepared Ti-MCM-41, but they did not report any catalytic data over these solids. Reddy et al. [7] also reported the possibility of preparing vanadium-containing MCM-41, active in oxidation reactions.
158 Very recently, Tanev et al. [8] have shown that mesoporous silicas (MS) could be prepared using a neutral templating route with primary alkyl amines as surfactant. A great advantage of the recipe was that the template could be removed from the mesopores by a solvent extraction, which is of great interest for environmental protection. We have followed a similar procedure to prepare Ti and V-containing mesoporous silicas. The influence of synthesis parameters, e.g. the metal content, the amine chain length or the synthesis time have been examined. These materials have shown very interesting properties as catalysts in oxidation reactions with organic peroxides as compared to zeolitic materials. 2. E X P E R I M E N T A L Ti or V-MS were prepared at ambient temperature by mixing a first solution containing tetraethyl orthosilicate (1 mole), ethanol (6.5 moles), isopropyl alcohol (1 mole) and the metal precursor (tetrabutyl orthotitanate or vanadyl acetylacetonate) to a second solution containing the alkylamine (0.3 mole) in water (36 moles). The resulting solution was homogeneized, stirred for about 30 min and aged for different periods at room temperature under static conditions. Solids were then filtered, washed several times with distilled water and air dried. Calcination of the samples was performed at 650 ~C in air for 6 h. When the organics were removed by a solvent extraction, 1 g of dried solid was dispersed in 100 ml of ethanol and the mixture refluxed for about 1 h. The solid was recovered by filtration, washed with cold ethanol and the procedure repeated once. A Ti-Beta sample was synthesized following the recipe of Camblor et al. [9] and contained about 1.5 wt % Ti and 0.4 wt % AI. A TS-1 sample was also synthesized following the patent literature [10]. Samples have been characterized using X-Ray diffraction (Philips PW 1710, CuKa radiation), IR spectroscopy (Perkin Elmer 580), U.V-Vis spectroscopy (Perkin Elmer Lambda 9) and EPR (Varian, E9). N 2 adsorption/desorption isotherms were carried out on a Catasorb apparatus. 3. R E S U L T S AND DISCUSSION
3.1. Synthesis and Characterization A series of samples have been synthesized with dodecylamine (n = 12 carbon atoms) and varying the amount of metal precursor in the gel. Gels were aged for 12 h
159 before recovering as-synthesized solids by filtration. As shown in Table i, the amount of metal incorporated in the silica matrix is very close to that introduced during the preparation. Table i Characterization of the different samples Sample Gel .
.
M~
oc
Si/Ti Product .
S(m2/g) .
m
.
973
r
V(cm3/g)
.
.
26.5
0.52
Ti-MS
i0()
85
i086
28
0.62
Ti-MS
50
45
i 066
29
0.65
I1-M~
30
3i
894
28
0.54
Ti-MS
20
i 9.5
667
25
0.36
V-Mb
i00
108
998
28
0.55
V-MS
50
62
i0 i5
28
0.64
V-MS
30
36
794
28.5
0.48
9 p()~) is the mean pore diameter V(cm3/g) is the porous volume measured at P/P0 = 0.5 in the N 2 isotherm. This suggests that all the Si and Me precursors were in the solid phase as the yield in Ti or V-MS was always very high (> 95 %). For relatively low Me contents (< 2 wt %), U.V-Vis as well as EPR spectroscopies showed that the cations were highly dispersed in the solid. Ti-MS materials exhibited a U.V. absorption band around 240 nm. The absorption edge decreased by about 10 nm to 230 nm upon calcination in air. For V-MS, EPR parameters were characteristic of vanadyl ions in an axially symmetric crystal field (A ![ = 190 G, g [] = 1.94, A__k_ = 72 G and gA_ = 2.00). The totality of the EPR signal disappeared upon calcination of V-MS samples in air. Dried calcined samples were white, but their color rapidly turned to bright yellow upon exposure to air, suggesting a change in the cation coordination. This was clearly evidenced in U.V-Vis and 51V NMR spectra. In dry samples, V 5 + cations are more likely in a tetrahedral environment but water molecules can easily enter their coordination sphere to give hexacoordinated cations. The process was perfectly reversible as original U.V-Vis and NMR spectra were restored after outgasing the samples at 200~
for 3 h. This clearly showed the relatively
160 high hydrophilic character of mesoporous silicas as compared to substituted zeolites like TS-1 or VS-1. All calcined samples exhibited relatively high surface areas, typically 1000-1200 m2/g and a mean pore diameter close to 28/~. Both slightly increased with the metal incorporation up to about 2 wt % of metal in the solid. Beyond that limit, for higher Me contents, the surface area as well as the pore diameter decreased. In the same time, U.VVis and NMR spectra revealed the presence of extrawall dispersed oxide species in the samples. However, the decrease in pore diameter could also arise from a loss of thermal stability of the structure for high Me incorporations. Similar observations have been made by Franke et al. [6] for Ti-MCM-41, and the authors interpreted the decrease in pore dimensions to the presence of extrawall species. A sample has been prepared with Si/Ti = 100 in the precursor gel and aged at room temperature for different periods ranging from a few minutes to 18 h. Indeed, Chen et al. [11] had reported that even though an X-Ray powder pattern typical of MCM-41 could be obtained after heating a silica-alumina gel at 70~
for 3 h, the
material was not thermally stable and collapsed upon calcination in air at 540 ~C. Table 2 clearly shows that using the present synthesis route, Ti-MS was obtained after a few minutes after mixing of all the reagents. There was no significant evidence for modifications occuring during the aging period ; the Ti content as well as the BET surface area and the pore dimension remained unchanged. The same observations could be made with vanadium-containing samples. Table 2 Characterization of Ti-MS samples recovered at different time intervals t(h)
Si/Ti
S(m2/g)
~p()~)
0
93
1081
28
0.58
1
85
1212
28
0.62
2
96
1091
28
0.60
3
94
1112
28
0.63
6
92
1174
28
0.62
18
85
1085
28
0.62
For the definition of ~p and V, see Table 1
V(cm3/g)
161 it has been widely reported that the pore dimension of MCM-4i synthesized with aikyitrimethyiammonium cations depended on the number of carbon atoms of the alkyi chain. For pure silica materials, data from Beck et ai. [3] showed an almost linear increase in the pore diameter from i8 ~ with octyiamine to about 37 /~ with hexadecyiamine. Very recently, Tanev et ai. [8] also reported that the pore dimensions of mesoporous silicas prepared using a neutral templating route increased with the amine chain length. For both Ti and V-substituted materials, we also observed that the dimension of the mesopores increased from about 25 ~ for n = i0 carbon atoms to 35 for n = i6. The corresponding isotherms are shown in Fig. i.
(c) o') A
I...03
1I~176
/
(b)
E "6 ..Q L_
o
Ca)
"13 <
E
0'
'
' 0.2
'
' 0.4
'
' 0.6
'
0'8.
'
I 1.0
plpo Figure i. N 2 adsorption/desorption of Ti-MS synthesized with CnH2n + i N H 2. n = i0 (a), n - i2 (b) and n - 16 (c)
162 These values are somewhat higher than those of Beck et al. [3] but also than those of Tanev et al. [8] who prepared their samples following a very similar recipe. As for MCM-41, the use of an amine with 18 carbon atoms led to materials with the same pore dimensions as those prepared with hexadecylamine. Another interesting parameter in the synthesis of mesoporous silicas is the surfactant/silica (Surf/SiO2) ratio. Beck et al. [3] have reported that hexagonal phases could only be prepared for Surf/SiO 2 < 1.1. For higher ratios, a cubic phase MCM-48 or unstable lamellar materials were obtained. We have synthesized a series of Ti-MS with Si/Ti = 100 in the gel and varying the Surf/SiO 2 ratio from 0.13 to 1.1. Whilst the surface area was high for relatively low ratios (< 0.5), it decreased to 350 m2/g for Surf/SiO 2 = 1.1 (Table 3). X-Ray diffraction showed that the cubic phase similar to MCM-48 was never formed, at least at a significant level. In contrast to the surface area and porous volume, the pore diameter increased continuously with the amount of amine introduced in the gel. These experiments clearly demonstrated that the best materials were obtained for Surf/SiO 2 ratios close to 0.3. Table 3 Characterization of Ti-MS synthesized with hexadecylamine and various Surf/SiO 2 ratios Surf/SiO 2
Si/Ti
S(m2/g)
~p(*.)
V(cm3/g)
I).13
81
968
34
0.59
I).27
85
1045
34
0.70
I).54
76
887
35
0.39
[).81
90
526
36.5
0.21
1.1
41
354
37.5
0.14
For the definition of ~p and V, see Table 1
3.2. Catalytic experiments Because of the high dispersion of Ti and V cations in mesoporous silicas, these materials are potentially interesting catalysts for the oxidation of large substrates with alkyl peroxides in the liquid phase. Ti-MS have been used as catalysts in the epoxidation of cyclohexene with both aqueous H202 and tert-butyl hydroperoxide (TBHP). The performances are compared with those of TS-1, that is known to be inactive in these
163 reactions because of restriction limitations, and Ti-Beta prepared following the recipe given by Camblor et al. [9]. Results are summarized in Table 3. With hydrogen peroxide, the activity of Ti-MS is very high as compared to those obtained over TS-1 and Ti-Beta. With TBHP, activities over Ti-MS and Ti-Beta are similar but the nature of the products formed differ considerably" because of the presence of aluminium in Ti-Beta, the diol derivatives is the major product formed whilst a selectivity in epoxide close to 9(1% is reached over Ti-HMS. This makes these materials particularly interesting for the selective epoxidation reactions with organic peroxides in the liquid phase. Table 3 Oxidation of cyclohexene over various Ti-containing catalysts Catalyst
Oxidant
COx(%)
SEp(%)
SD(%)
TS-1
H20 2
16
97
3
Ti-Beta
H20 2
77
2
98
Ti-MS
H20 2
95
79
21
Ti-Beta
TBHP
92
90
10
Ti-MS
TBHP
97
88
12
COx is the conversion in oxidant, SEp the selectivity in epoxide and SD that in diol. Reaction conditions "0.1 mole cyclohexene, 20 ml ethanol, H202/cyclohexene = (}.2, T = 7{1~C. Data obtained after l h30 of reaction. The same catalysts have been used for the oxidation of substituted anilines. Over all Ti-containing catalysts, aniline was converted selectively into azoxybenzene with a selectivity close to 95 %. The activity over Ti-MS was comparable to that over Ti-Beta, and both were very high as compared to that obtained over TS-1. Over V-MS materials, the only product formed was nitrobenzene, but the catalysts were only active with TBHP and conversions relatively low. Interesting differences between Ti-MS and Ti-Beta were observed during the oxidation of 3-chloroaniline.
CI
,.,,,vmw2r'2~
CI
0
CI
164 The selectivity in 3-3' dichloroazoxybenzene was only 6() % over Ti-Beta after 2 h 30 of reaction whereas it was already 95 % over Ti-MS after 15 min. In both cases, all the H 2 0 2 introduced at the beginning of the reaction had been consummed. This example clearly evidenced the advantage of mesoporous systems with respect to zeolites in the liquid phase oxidation of organic molecules. 4. R E F E R E N C E S
1
G. Perego, G. Bellussi, C. Corno, M. Taramasso, F. Buonomo and A. Esposito, Stud. Surf. Sci. Catal., 28 (1986) 129.
2 3
B. Notari, Catal. Today, 18 (1993) 163. J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T-W Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins and J.L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834.
4
S. Inagaki, Y. Fukushima and K. Kuroda, J. Chem. Soc., Chem. Commun. (1993) 680.
5
A. Corma, M.T. Navarro and J. Perez-Parient6, J. Chem. Soc., Chem. Commun. (1994) 147.
6
O. Franke, J. Rathousky, G. Schulz-Ekloff, J. Starek and A. Zukal, Stud. Surf. Sci. Catal., 84 (1994) 77.
7
K.M. Reddy, I. Moudrakovski and A. Sayari, J. Chem. Soc., Chem. Commun.
8 9
(1994) 1059. P.T. Tanev and T.J. Pinnavaia, Science, 267 (1995) 865. M.A. Camblor, A. Corma and J. Perez-Parient6, Zeolites, 13 (1993) 82.
10
M. Taramasso, G. Perego and B. Notari, US Pat, 4 410 5[)1 (1983).
11
C-Y. Chen, H-X. Li arid M.E. Davis, Micorporous Mater., 2 (1993) 17.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 1995 Elsevier Science B.V.
165
Bimodal porous materials with superior adsorption properties C. J. G u o
National Centre for Upgrading Technology Western Research Centre, CANMET, 1 Oil Patch Dr., Devon, Alberta, T0C 1E0, Canada ABSTRACT Porous materials with bimodal (micro and meso) pore size distribution have been prepared at ambient conditions. The materials contain randomly distributed mesoporous channels with uniform pore size and exhibit very large surface areas and pore volumes. The adsorption properties for water and some large organic molecules of the materials were determined. The water sorption capacities of the materials are about 300% higher than those of conventional zeolite molecular sieves such as zeolite 13X. The materials also have a great capacity to adsorb large molecules (e.g., > 60 wt. % tetralin) that zeolites exclude. The open structure and large pore size also result in high rates of adsorption and desorption. The superior adsorption properties of these new materials indicate their great potential for applications in adsorption and catalysis. Large-scale production of the mesosieve materials is expected to be straightforward and economical. INTRODUCTION There is a large and growing demand for adsorbent materials for use in various industries. The major commercial adsorbent materials on the market today are aluminas, molecular sieve zeolites (A, X, and mordenite), silica gels, carbons, and organic polymers. Compared with the other adsorbents, zeolite molecular sieves have significantly higher sorption capacities at low partial pressures. The maximum sorptive capacity of zeolite 13X which has the highest capacity among zeolites, is 25 to 36% [1]. A key determinant of the adsorption properties of a porous solid is its microstructure. A porous solid with high adsorption strength at low partial pressure, high capacity at high partial pressure and with rapid adsorption and desorption rates would be an ideal material for adsorption applications. CANMET has recently developed a novel method to make porous material with just these features [2]. The water sorption capacity of this new material is about 120 wt. %, which is 200 to 300 % higher than most of the commercial adsorbents currently on the market. The preparation and projected large scale manufacturing procedures are simple since only ambient
166 conditions are involved in the original preparations. In this paper, the adsorptive properties of the uniquely structured materials and some characterizations of their micro structures are presented. MATERIAL CHARACTERIZATION Researchers in Mobil R&D corporation had developed crystalline mesoporous molecular sieves designated as M41S using high temperature (100 to 200 ~ hydrothermal conditions (4,5). The present materials were all prepared using ambient conditions (0 to 25 ~ and atmospheric pressure) and short times (5 minutes to 4 hours) followed by a thermal treatment procedure. Silicate and aluminate sources common in zeolite synthesis and commercial surfactants such as Ammonyx KP (oleyl dimethyl benzyl ammonium chloride, Stepan Co., IN) were used in the preparations. The details of the preparation procedure and compositions are not described here. The major features of these materials are high porosity, low particle density, high surface area, and high pore volume. The surface area (S) and pore volume (V) of the materials, as well as the relative amounts of micropores and mesopores can be varied as required (from 100 to 1200 m2/g for S, and from 0.1 to 1.3 cm3/g for V) by controlling the original mixture composition. Commercial manufacturing of the material in a continuous mode is easily achievable because of the simple procedures required: ambient conditions, a short amount of time, and a final thermal treatment in a regular furnace. Figures 1 shows a SEM (Scanning Electron Microscopy) micrograph of a typical
Figure 1. A SEM micrograph of the mesoporous materials.
Figure 2. A TEM mesoporous particle.
image
of
167
sample of the new materials. It is clear that the material is composed of small particles with diameter of less than 0.5 micron. These small particles themselves are highly porous as indicated by their high surface area. Figure 2 is a TEM (Transmission Electron Microscopy) image of the same sample. It is evident that different from most zeolites and crystalline mesoporous sieves such as MCM-41 which has a well organized hexagonal pore structure, the present materials contain randomly distributed channels with uniform mesopore size (about 3 nm for this particular sample). The micropores are not visible on the TEM image but are believed to be in the walls of the mesopores. As can be seen from the pore size distribution from nitrogen adsorption in Figure 4, in the mesoporous range, most of the pore volume is contributed by pores with a diameter of 3 nm. Comparing the results of figures 2 and 4, there is a good agreement on the channel size of the material between the two independent characterization methods. This agreement implies that the new materials, which are not really crystalline, have randomly distributed channels with a uniform mesopore diameter of 3 nm. The name mesosieve is used for these new materials in the rest of the paper. In addition to the regular mesopore size, the materials also have very large surface area and large pore volume. Table 1 lists some typical physical properties of the materials compared with zeolite 13X. The framework density was measured using helium and the particle density (or mercury density) is calculated from the framework density and N 2 saturation capacity. The materials are stable under severe acidic and thermal conditions; there was no pore structure change and only a 3 % surface area decrease was observed after a sample was placed in 70% nitric acid for five days and then calcined at 510 ~ Calcination at 800 ~ for two hours would not significantly change the pore size distribution pattern although a less than 20% decrease in surface area was observed. Table 1. Some physical properties of a mesosieve and zeolite 13 X Sample ID
Skeletal density (g/cm3)
Particle density (g/cm3)
Surface area (m2/g)
Total pore volume (cm3/g)
Mesosieve 11195A
2.39
0.63
1075
1.36
Zeolite 13X
2.03
1.31
790
0.32
ADSORPTION P R O P E R T I E S OF THE MATERIALS Figure 3 compares an N2 adsorption isotherm of one sample of the new materials (Figure 3a) with that of zeolite 13 X (Figure 3b). As is evident from the figure, the new mesosieve exhibited a type IV isotherm and 13X a type I isotherm. At a relative pressure of 0.001, 85 % of 13X total capacity is occupied because of the strong adsorption potential in
168
1
i
i
i
l
i
+
I
T
................ i .......I........I....... I........t.......I........t.......T
!" - I :
'dt
~ 'i
........ ,........ ! ~l....... .+........ , , , + / ~ ~ ~ ,
+
!........ l..-,..+,.
++B} + ............... i +....... i ........ +....... +........ +....... i ........ l
....... !........ t ....... j .... //,,.. ..... l ........ l ....... +........ +....... +........ i ..............
I I ........ +!...... ~ ,
! ,P" i
i
~
l ~ ~
i
i
i
l
i
~
+....... Ii...,
'~"i
. . . . . . . .
....... +........ i....... + v o = ] _ p
'
'
;
"
~ S
I
I
i
i
l d,, = 28.
%
o
./-----i ........ i ....... i ........ i ....... i-~
:
,
%
, o.,
,
,
=
,
o
%
\~2 ~
,
, , ,
%
%
.
:.
I. . . . . . .
t+ .t....t .
--
:j!io,-.o,,~
I I"]:
%
"o
~v
,.,=--,--!
-.,
o
%
l
l
i
Zeolite 13X:i .... , ....
.......
+Vp
=
0.32
l
..+....... +s=798
r=o,,./
+'-'L--'-~--,., -o
+
l
i
L , o L I ! L ! ! ! ! %
l
'[ .......]
,
.... l---t.J...
.
-+ ....... +........ +....... i ........ +....
!
.... il
1235
=
,,
. ;7 ...,.. 7"i 711 IT 71i+.~ . ; . '
!
.....
".
.......................................
:
i
-,....
l ....... ] ........ +....... +........ +....... +........ l:~,..~i
........ ~
~I
.
,~.......j_..
%
+....
i
i do = 5 -
+
+
+
+
%
%
%
%
7{
+ !
Relative pressure F i g u r e 3. N i t r o g e n sample
13X
sorption
isotherms
of a mesosieve
sample
(3a) a n d a z e o l i t e
(3b).
the zeolite micropores. The sudden jump in adsorption capacity at middle relative pressure on the isotherm of the mesosieve is a result of capillary condensation in the mesopores. The high "knee" in Figure 3a also indicates the presence of a significant micropore volume in these materials. It can be seen that the first "knee" sorption capacity of the mesosieve is already as high as the saturation capacity of zeolite 13X. The total sorption capacity of the new material is actually about four times that of 13X as can be seen from Figure 3. Such large differences in pore volume will be reflected in adsorption capacities.
......
..J ....... -~- ...... i ........ i ......... . ................ ] ................ + ................
i ................. o.~
i
i
i
i
i
i
~ . . . . . . . ~. . . . . . . . ~. . . . . . . . i . . . . . . . . i . . . . . . . . ".-. . . . . . . .'.L. . . . . . . . . . . . . . . .
.............
~. . . . . . . .
i
i
{
{
i
i
i
t
1. . . . . . . .
i ........
; ........
i ........
~.......
~. . . . . . . .
! ........
l
;H-K~
i
i
i
!
i
i
i
i
i
i
~,:,::, i iiii!i 0:m II ', ',',:', "~ 0 . . ; ~ '., ',;:; . . . . . . . . . . . II
~,,:,,::! Ii li
/ .~
,~i
0.~. ....... ~ .I--~--,
. . . . . . . ~. . . . . . . . i . . . . . . . . i . . . . . . . . i . . . . . . . . .; . . . . . . . -!.. . . . . . . . .;. . . . . . . .
To
9
;
i
..,1 ....... : ....... ~ o.= ..................
i
i
+
+
+
i
i
i
i
U
' ........
i ........
9.
.
.
i .
I , I i i I
i I iii i|lll
. . . . . . . . . .. .. . . . .
i I , I,
i
i
.
.
.
.
.
0:04
.
It
IIIII
II
I IIII I IIII
i I illl i I i ill i i i i1|
I all I
i
i
i
Figure
4. The
pore
models
size d i s t r i b u t i o n (HK and DFT).
I
I
I i IIII i i illl
i
I I ]J
I IIIII I i i iii i i illi
+ i i
* I i I i I
i
i
I I I
D F T ....... .......
I!'!1
. . . . . . . . . . . . . . . .
I
Iiiii
I I IIII
'
P"I '''"' I I IIII I i illl i ! {ill
I
I
I
'
' ' '''"'
I I !
I I !
I I !
I
I IIIII I I llil I I ~ III
II. ,I,,,,,, ,,,,,,
,
, , ,,,,,,
I i i
I i i
I IIIIIII I I IIII , iiiiiiii ,I i i i i i |111111 ii i i i i i
', ]
'~" I
~..I
I00
I i i i
,,.i IIIII 131111
IOO0
Pore diameter(A) of the
mesosieve
as d e s c r i b e d
I
"!
I IIIIII i i i i i ii i iiiiii
I IIIIl~llllhllllllllll I~11+~ I ~ 1 I I I I IIIII I I III IIIIIIII111111111 I I I I I 1 ~ 1 ~ ~ 1 II i ii iiiii!111 IIIIIIllllllllLqll I II IIIIIIIIrll II I III Iil IH II
IO
',
IIIII
III
Pore diameter(A)
adsorption
| ! ~ I
II IIIII
9
i
, .
,i,,,i
II I
i
| iI||l I i IIII
I I l IIII
o.~ , ..... i,,~-O',',', .... ~ ...............
o.~
I I
.
I IIIIII - I - . - - . 4 - - ~ l l Il ~ I I I I ~ 1111.1.
, ,,, ,, III
0.00
| I
, I I
i llll
,,
~ ;,
...................
..i ....... i ....... J........
.... ~........ +........ +........ ~........ " ....... + ....... , ........
"........
i i iii
,,
',',',:',:,, ........... ... . . . . . . . .
by two
169 In Figure 4, the pore size distribution of a typical mesosieve is described using two adsorption models, the Horvath-Kawazoe (HK) model [6] and the density function theory (DFT) [7], using nitrogen adsorption data. The DFT claims applicability to both microporous and mesoporous ranges although its accuracy in modelling nitrogen adsorption in micropores of diameter smaller than 1 nm is questionable. It is clear that the new materials have a bimodal pore distribution, with a significant presence of both micropores and mesopores. The micropores are in the range of 0.6 to 1.0 nm whereas the mesopores are all larger than 2.5 nm. Such bimodal pore size distributions are a very positive feature for the materials used as adsorbent since the micropores provide a strong adsorption potential at low partial pressures, whereas the mesopores assure very large sorption capacity at higher relative pressures. To demonstrate this effect, adsorption experiments were conducted to measure both the total capacity and adsorption rate at low partial pressures and short times. Figure 5 compares the saturation capacities for water, cyclohexane, and tetralin of several mesosieve samples with those of zeolites 5A, ZSM5, and 13X. The sorption capacities were determined by exposing a dry sample to the saturated vapor of an adsorbate at 23 ~ and weighing its equilibrium mass at the same temperature. Compared with 13X particularly, the mesosieves showed more than 300% higher water sorption capacity, more than 400% higher cyclohexane sorption capacity, and close to 300% higher tetralin sorption capacity. Compared with zeolite 5A, the mesosieve water capacity is 350% higher, cyclohexane capacity 1000% times higher, and tetralin capacity 3400% higher. Such extraordinarily high sorption capacities are a result of the large mesopores and high pore volumes of the mesosieves. Another possible advantage of the micro-mesopore combination is that a molecular sieving effect on molecules of size 0.6 to 1.0 nm can be provided by the micropores whereas the mesopores 140 assure a small diffusion resistance and a large volume for molecular transport. 120 El Water I [ ] Cyclohexane
In addition to the saturation capacity, the sorption rate of a particular adsorbate in the mesosieves is significantly higher than that in zeolite adsorbents. In Figure 6, two adsorption uptake curves from the adsorption of water in a mesosieve and in zeolite 5A, both in 1/32" extrudate form, are compared. This experiment included placing a dry sample in water-saturated air at room temperature and monitoring the sample mass change with time. The mesosieve shows faster water uptake rate and higher capacity. In Figure 7,
"~100
"o
[] Tetralin
i!~d ill.'
~o 80
~U,i
-o 60 C
=
~
40
o
/ 5A
ZSM-5
13X
MS-A
MS-B
~Hm
MS-C
Sample ID
Figure 5. Comparison of adsorption saturation capacities for three vapors of three mesosieve samples (MS) with that of zeolites 5A, ZSM5 and 13X.
170 the desorption curves of water desorbing from a mesosieve sample and a 13X sample under the same conditions are illustrated. The faster desorption in the mesosieve is evident: at the end of two-hour desorption, more than 60% of the total amount adsorbed is desorbed from the mesosieve, whereas only 26% is desorbed from 13X; this is on the top of a 300% higher total water loading. The desorption experiment was conducted by exposing a water-saturated sample to air and monitoring its mass change at room temperature. Obviously, the open pore structure and the presence of mesopores resulted in the high capacities and faster diffusional mass transfer rates. 35 f
70
A 30
~2s 'U o
"~ 40 m " 30 ,,,3 9 ,,9 "-o 20
t~ 2 o 0 Ir
9a 15
m
e~ 0=
10 5
I 013195A --4113Xzeolite
'ID , 960 .e oM ,, 50 "o
~"
MS(run 2) 11 10
20 30 Time ( m i n . )
40
50
Figure 6. Water adsorption c u r v e s o f a m e s o s i e v e and a zeolite 5 A s a m p l e .
0
20
40
60
80 100 120 140
T i m e (rain.)
Figure 7. W a t e r desorption c u r v e s of a m e s o s i e v e and a zeolite 1 3 X sample.
CONCLUSIONS Highly porous materials with bimodal (microporous and mesoporous) pore size distribution were prepared at ambient conditions and using short preparation times. The materials contain randomly distributed channels with uniform mesopore size. Large-scale production of the materials is expected to be easy and economical. The important features of the new materials are: 1. Unique pore structure, possibly micropores connected to uniform mesopores. 2. High surface area (up to 1200 m2/g and can be varied). 3. High pore volume (up to 1.3 cm3/g and can be varied). 4. Small particle size and easily formed into extrudates or tablets. 5. High stability under severe thermal and acidic conditions. 6. Low apparent density (0.6 to 0.7 g/cm3).
171 7. Noncrystalline. The new mesoporous materials exhibit extraordinarily high adsorption capacities for both water and organic compounds. Their water sorption capacities are 300 % higher than zeolite 13X and they adsorb large molecules like tetralin (which conventional zeolites exclude) in large quantity ( > 60 w. %). The materials also show greater rates of adsorption and desorption than zeolites. The unique pore structure of the materials indicate great potential for applications in adsorption and catalysis, particularly for applications that require 1) large pores and high surface area and 2) both micropores and mesopores, small mass transfer resistance and large pore volumes. REFERENCES
.
.
.
.
7.
R. H. Perry and D. H. Green (eds.), Perry's Chemical Engineer's Handbook, McGraw-Hill, Inc., 16-9, 1984. C. J. Guo and C. Fairbridge, CANMET division report WRC 93-48 (CF), November, 1993. C. T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710. J. S. Beck, C. T-W. Chu, I. D. Johnson, C. T. Kresge, M. E. Lex~nowicz, W. J. Roth and J. C. Vartuli, US Patent 5108725, April, 1992. G. Horvath and K. Kawozoe, J. Chem. Eng. Jpn., 16 (1983) 470. J. P. Olivier and W. B. Conklin, "The international Symposium on the effects of surface heterogeneity in adsorption and catalysis on solids", Kazimierz Dolny, Poland, July, 1992.
This page intentionally left blank
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviot and S. Kaliaguine (editors) 1995 Elsevier Science B.V.
173
M C M - 4 1 t y p e silicas as s u p p o r t s for i m m o b i l i z e d c a t a l y s t s Daniel Brunel*, Anne Cauvel, Francois Fajula and Francesco DiRenzo Laboratoire de Mat~riaux Catalytiques et Catalyse en Chimie Organique, CNRS-URA 418, Ecole Nationale Sup6rieure de Chimie, 8, rue de l'Ecole Normale, F-34053 - Montpellier C6dex 1 - Fax: + 33 - 67 14 43 49 Abstract MCM-41 type silicas were covalently grafted with various functional alkoxysilanes (RO)3Si(CH2)3 X with X = C1, NH(CH2)2NH2 and NHC(O)NSalpr. The functions of the first two organic moieties already attached were further transformed into respectively 2-(NHCH2)Pyr, 4-(NH(CH2)2NHCO)Pyr also known as organic ligands of transition metals. The grafted mesoporous silicas were c h a r a c t e r i z e d by IR, MAS-NMR s p e c t r o s c o p i e s , thermogravimetry, nitrogen adsorption and elemental analysis . The coupling reactions of organic ligands do not modify the covalent grafting bonds. Pore opening shrinks at increasing organic coverage. The diameter of the channels accessible to nitrogen varies from 33 to 13 /~. A total surface lining by concentrically oriented organic chains is suggested by the decrease in the nitrogen adsorption enthalpy as a function of the organic coverage. 1. INTRODUCTION MCM-41 molecular sieves are a new class of mesoporous aluminosilicates featuring cylindrical regular mesopores of monodispersed diameter w i t h potential applications in catalysis and adsorption [1,2]. They are obtained by precipitation of amorphous silica-alumina in the presence of cationic surfactants. The pores of the MCM-41 type materials are templated by the surfactant micelles. While the hydrocarbon chain length of the surfactant rules the pore diameter, the conditions of the hydrothermal synthesis, in particular the alkalinity of the parent hydrogel, influence the wall thickness [3]. An increase in the pore spacing leads to an improved thermal stability of MCM-41-type materials. Pure silica MCM-41s can also be prepared and they feature a better stability than their silica-alumina analogs. MCM-41-type silicas were obtained with a pore diameter of 33/~ and wall thickness higher than 10/~. MCM-41 type silicas are an ideal raw material for the design of new mesoporous solids having adjustable chemical and physicochemical properties [4] in view of applications in the field of adsorption and fine chemical catalysis. This objective can be reached by lining of the mesopore surface with covalently attached transition metal liganding moieties. The volume available inside the MCM-41 mesopores is much larger than in the channel volume of the usual
174 zeolite catalysts. The insertion and grafting of bulky, sterically-hindered functional molecules is hence possible, without a decrease of the accessibility of the catalytic groups. As the mesoporous surface of the MCM-41 type silicas presents the same surface silanol groups than the traditional amorphous silicas, it can be modified by applying usual methods of silica functionalization. They deal with the covalent linkage of organic groups to the silica surface by condensation of organotrialkoxysilanes with the silanol groups [5-22]. We report here the anchoring of organic groups to MCM-41 type silicas using functional propyltrialkoxysilanes. The organic moieties were f u r t h e r transformed by coupling reactions with suitable organic ligands of transition metals. Our goal in preparing these materials was to obtain mesoporous solidbound ligands that yield systems with potential for catalytic oxidation of organic substrates. As most of the monodentate ligands used to immobilize transition-metal catalysts suffer from the disadvantage of the metal complex leaching into the solution, there is considerable interest in covalently attaching multidentate chelating agent to a support surface. For this purpose, we selected the following l i g a n d s : (pyridino-2-methyl)amine, (2isonicotinamidoethyl)amine and pentadentate Schiff base as SalDPT [23,24]. In the case of the two first ligands, mild coupling organic reactions were carried out to perform the coupling of the liganding moieties while avoiding alteration of the covalent grafting bonds. The different modifications were controlled at each step using various characterization techniques. This study allowed the determination of the new adsorption properties of the modified mesopore surfaces. 2. E X P ~ A L 2.1. MCM-41 silica.
Pure MCM-41 mesoporous silica (MPS) was prepared in the presence of cetyltrimethylammonium hydroxyde according to the method described in the literature [1,2]. The MPS material consists in SiO2 containing 0.003 A1/(AI+Si) and 0.0014 Na/(AI+Si). X-ray powder diffraction pattern matches well with the patterns reported by J.S. Beck et al [2], with d loo = 40.0/~. The hexagonal lattice parameter is equal to 46.2 /~. The nitrogen sorption isotherm of MPS is a classical example of type IV isotherm [24], showing monolayer and multilayer adsorption on a mesoporous surface of very high area and a sharp, reversible step at P/P0 0.38, characteristic of capillary condensation within the mesopores (vide infra). No hysteresis loop is observed due to the low filling pressure of the small mesopores.
2.2. Functionalization procedure 3-chloropropylsilylated-MPS (C1-MPS), 3-(2-aminoethyl)aminopropylsilylated -MPS (NH2EtN-MPS) and 3-(bis-[3-(salicyliden-amino) propyl])carbamatopropyl silylated-MPS (SalDPT-amido-MPS). A suspension of freshly activated MCM-41 silica in toluene was refluxed and stirred for 1.5 hr. with the corresponding functional organoalkoxysilane under dry nitrogen atmosphere. After distillation in a Dean-Stark collector of a fraction of toluene containing volatile compounds, the mixture was again heated at toluene refluxing temperature for 1.5 hr. The distillation and heating sequences were repeated. After cooling, the solid was extracted in a soxhlet
175 apparatus overnight with ethyl ether and dichloromethane, then evacuated under vacuum at 200~ for 6 hr. Elemental analy~i~: C1-MPS: C 6.34%, C1 3,29%; NH2EtN-MPS" C 15,23%, N: 6.06%; SalDPT-amido-MPS: C 26.36%, N 5.17%.
2.3. Modification of the functional group 2.3.1.3-(2-pyridinomethyl)aminopropylsilylated-MPS (Pyr MeN-MPS) A suspension of activated C1-MPS material in toluene was refluxed and stirred in an excess of 2-(aminoethyl)pyridine for 6 hr. After separation, the modified solid was extracted according to the previous procedure, then dried under vacuum at 180~ overnight. Elemental analysis: C 14.62%, N 3.89% 2.3.2. 3-(2-isonicotinamidoethyl)aminopropylsilylated-MPS (IsoNicEtN-MPS) Activated NH2EtNH-MPS in suspension in dichloromethane was refluxed and stirred with an excess of a mixture (1/2) of isonicotinic acid and N,N'dicyclohexyl carbodiimine for 6 hr. The modified solid was then separated, washed in succession with water, ethanol, then treated according to the previous procedure. Elemental anolysi~: C 23.05%, N 6.98%. 3.3. Characterization Analyses of the modified solids were made using 13C MAS-NMR, Infrared and UV Spectroscopies, Thermogravimetry, Nitrogen Adsorption and Desorption Isotherm and Elemental Analyses. RESULTS AND DISCUSSION The grafting reactions on the MPS support were studied first by infrared and 13C MAS-NMR spectroscopies. Infrared spectra of the modified mesoporous silicas show a band at 2940 cm -1 characteristic of-CH2- stretching vibration whereas the band at 2970 cm-1 associated with the CH3 of the ethoxy group has a much lower intensity than in the grafting agent spectrum. Moreover the grafted MPS spectra exhibit lower silanol band intensity at 3741 cm -1 than the parent MPS. The release of ethanol, detected and characterized by GCMS during the process confirms the formation of the Si-O-Si linkage according to the following reaction scheme: ~-OH
,,, (EtO)3Si(CH2)3X
~
NN[_O\ S i / ~ / ~ X]---O/
X
+ 2 EtOH
X= CI, NH(CH2)2NH 2, NHC(O)SalDPT 13C MAS-NMR spectroscopy allows the determination of the structure of the grafted hydrocarbon chains. The assignments of the 13C NMR signals of the modified mesoporous silicas are reported in Table 1.
176 Table 1 13C CP-MAS NMR spectral features of the grafted mesoporous silicas Grafted species
Ca
C~
Cy
N(CH2)nN Aromatic C
-=SiCH2aCH2~CH2Y-CI
8.9
26
46
=_Si(CH2)3-NH(CH2)2-NH2
9.5 22.5
38
51
-Si(CH2)3-NHC(O)-SalDPT
9.5
22
40
45
118 131
-_-Si(CH2)3-NHCH2Pyr
10
19
38.5
52
125 138 149
=_Si(CH2)3-NH(CH2)2-NHC(O)Pyr 10
22
40
50
124
ppm
145
CO,CN
161
158
163
165
Thus, the eventual modification of the structure of the function can be monitored by the change in the 13C CP-MAS-NMR spectra resulting from the coupling reactions. This is examplified on Figure 1 showing the intensity of the signal assigned to the CH2-C1 group on the C1-MPS spectrum (Fig.la) at 47.2 ppm which is very low on the spectrum of the resulting Pyr MeNH-MPS (Fig. lb). Moreover this later spectrum exhibits other signals characteristic of the 2-pyridinomethylamino group. The disappearance of the residual ethyl arms during the coupling t r e a t m e n t probably results from nucleophilic assistance of siloxane coupling between adjacent chains.
=
S i ( O E t )
( C H 2 )
••-•• 3-CI
~.\ \ i ~ ~
-(CH1)3 - N I I - C I I .
1~o
.
_
,
.
.
1
-
,
6
--~
-
.
|
-
14o
.
.
,
- . -
,oo
,
-
.-
,
60
-
. - !
.
.
.
.
.
,
iO
PPM
Figure 1. 13C CP MAS-NMR of a)C1-MPS b) PyrMeN-MPS
PPM
Figure 2. a)13C CP MAS-NMR of SalDPT-amido-MPS. b) J-Mod. 13C NMR of SalDPT in CDC13 solution
On the other hand, Figure 2 illustrates the identification of the anchored
177 26,0 ~ SalDPT group attached with c a r b a m a t o p r o p y l silane chain (Fig 2a) by comparison with the s p e c t r u m of SalD PT zo.( material in CDC13 solution (Fig 2b). The diffuse r e f l e c t a n c e s p e c t r u m of SalD PT-amido-MPS presented on figure 3 is consistent with the s t r u c t u r e of the salen group linked by a carbamate function (~,= 254 14.( and 317 nm). The b a n d at ~,= 400 n m would K-M be c o n s i s t e n t w i t h excitonic t r a n s i t i o n r e s u l t i n g from a t i g h t ordered packing of 8. salen molecule. The i n f r a r e d s p e c t r u m of this solid is also in a good a g r e e m e n t with the proposed structure. This latter technique as well as 13C MAS-NMR spectroscopy also z. 200 300 ~0 500 indicate t h a t the coupling of organic ligands zi nm of t r a n s i t i o n m e t a l to the grafted molecules Figure 3. Diffuse reflectance spectrum does not a l t e r the covalent siloxane bonds of SalDPT-amido - MPS. between silica and organic moieties. Table 2 reports the organic content and coverage of the grafted mesoporous solids deduced from the elemental analysis and thermogravimetry.
Table 2. Organic coverage and content of modified MPS.
Materials Cl-MPS NH2EtNH-MPS PyrMN-MPS
Molar ratio C/Cl 6.1
chain nm 2. 0.6
10.3
-(ctl2) 3 -Nll-(Cll2)2-Ntt 2
C/N 2.7
1.3
23.5
"(C!]2)3 "NI]'CIt2 --~(,_))
C/N 4.4
0.9
26.7
C/N 3.8
1.0
33.5
C/N 5.9
0.6
40.7
Organic chain -(oil2)3 -ct
{or~) k SiO2
w
-(Cll2) 3 -NII-(CII2)2-Nlt
IsoNicEtN-MPS
SalDPT-amidoMPS
~,-~
oII -((;lt2)3 -Nn-C -N
llO
* surface area of the mineral support The organic coverage of the modified m a t e r i a l was c a l c u l a t e d from elemental analysis d a t a t a k i n g into account mass % chlorine for chloroalkyl
178 chain and mass % nitrogen for amino or amidoalkyl chain containing or not pyridino group. The organic content is obtained from thermogravimetric data as the mass loss at T > 200~ It is noticeable that the organic coverage is lower for C1-MPS than NH2EtNH-MPS. Probably the amino groups enhance the substitution reaction at the Si atom [25]. The low organic coverage of C1-MPS corresponds to a C/C1 ratio higher than the stoichometric value. It is likely that the C/C1 ratio is increased by the presence of EtO- groups linked to the Si atoms belonging to the grafted chain or to the surface. This hypothesis is consistent with the i.r. and 13C NMR results. It is noteworthy that C/N ratio confirms a complete coupling reaction whatever the previously grafted organic function. The nitrogen sorption isotherms of the functionalized MPS give informations on their texture and surface state. Figure 4 shows the isotherms of some materials grafted with chains of different lengths. Data derived from the sorption isotherms of all samples are reported in Table 3.
jf
8O0
n_
~=m600
j
v
w= 4 0 0 o
/
~
c 200 _1 o
.,,,..,.,.,,..~l~ ~ .
. -
450
400
300
l
200
100
0
,,~
o
~,
'
a.'2
]',, RS~..ATIV[
'
9
o'.6 PRESSURE
o'.~ ,
'
'
~
o
o
(J=/;=o)
.
0.2
.
.
o
u
Ri[LPTIV~
.
o
6
PRESSURE
o.~. ,
(P/Pro)
Fig.4. Nitrogen sorption isotherms of a) parent MPS b) (1) CI-, (2) PyrMN-, (3) SalDPTamido-, (4) IsoNicEtN-MPS. Table 3. Textural and thermodynamic parameters deduced from nitrogen sorption isotherms mesoporous mesoporous diameter BET Materials surface volume (cc/g) (A) parameter C (m2/g) MPS
920
0.76
33
100
C1-MPS
851
0.57
27
60
PyrMN-MPS
577
0.35
24
50
NH2EtNH-MPS
586
0.29
20
22
SalDPT-amido-MPS
608
0.31
20
19
isoNicEtN-MPS
436
0.22
13
28
179 The surface area and mesopore volume decrease with increasing length of the grafted chain, but the characteristic features of the MPS isotherms are essentially preserved. All isotherms are of type IV, indicating the preservation of the mesoporous system during the grafting reaction or the modification of the organic chain. However, the characteristic step of the sorption isotherm, corresponding to the Kelvin filling of the mesoporosity, becomes less sharp at increasing organic content, suggesting that the pore size distribution is widening. The pressure at which the step of the isotherm occurs decreases with increasing length of the organic molecules. The diameter of the organiclined mesopores can be evaluated by the ratio dmeso = 4V / S between mesopore volume and mesoporous surface area. The average pore diameter are reported in table 3. The pore opening shrinkage fits fairly well with the increase in the organic chain lengths. This trend is consistent with the variation of surface area and mesoporous volume. The application of the BET equation to the nitrogen sorption isotherms provides some useful information on the energy of the interaction between a probe molecule -nitrogen- and the surface. The BET parameter C is roughly connected to the nitrogen adsorption heat according to the following equation: C= exp[ (Eads- E1 ) /RT] where E1 is equal to liquefaction heat of nitrogen. Values of the parameter C for all samples are reported in Table 3. All organic-lined MPS feature much smaller values of the parameters C than the parent silica. The adsorption heat of nitrogen is indeed lower on organic surfaces than on hydroxyl-rich surfaces. As a consequence, the low C values for modified MPS can be considered as an indication of regular surface coverage by the organic groups. 4. CONCLUSION The MCM-41 type silicas provide suitable supports for anchoring organic moieties to the inner surface of a mesoporous system. The organic lined mesopores of regular, well-controlled diameter can be obtained by standard functionalization methods. The grafted function can be further transformed into well-defined transition metal liganding moities without loss of either the organic chain content or the regular mesoporous structure. Nitrogen sorption isotherms are useful tools to characterize the properties of such potentially hydrophobic materials. The strong decrease of the nitrogen adsorption heat with the organic coverage is a significant test of the modification of the surface properties. The decrease of the value of the C parameter of the BET equation indicates t h a t the mineral surface is no longer accessible to adsorbed molecules. These results confirm the unique properties of the composite materials prepared by grafting organic molecules to the inner surface of MCM-41 type silicas. Potential applications would be relevant to both specific oxidative catalysis induced by the anchored transition metal complexes and the hydrophobic property peculiar of the lined organic moieties. AI~OWLEDG~ The authors are grateful to ELF and CNRS for financial support. They thank Annie Finiels for her help in taking part of the 13C NMR spectra in
180 CDC13 solution. Anne Cauvel is indebted to ADEME (Agence de 1' Environnement et de la Maitrise de r Energie) for a doctoral grant. R~'ERENCI~ 1 J.C. Beck, C.T.-W. Chu, I.D. Johnson, C.T. Kresge, M.E. Leonowicz, W.J. Roth and J.C. Vartuli, to Mobil Oil Corporation, WO91/11390 (1991). 2 J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T.-W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCuUen, J.B. Higgins and .L. Schlenker, J. Am. Chem. Soc., 114, 10834 (1992). 3 N. Coustel, F. Di Renzo and F. Fajula, J. Chem. Comm., Chem. Comm., 967 (1994). 4 A. Cauvel, D. Brunel, F. DiRenzo and F. Fajula, "Organic Coatings" 53rd International Meeting of Physical Chemistry, Paris, 2-6 jan. 1995. 5 W. Hertl, J. Phys. Chem., 72, 1248 (1968). 6 B. Arkles, Chemtech, 766 (1977). 7 D.R. Fruge, G.D. Fong and F.K. Fong, J. Am. Chem. Soc., i01, 3697 (1979). 8 L. Yu Fu, X. Yong-Xia, X. Don-Peng and L.J. Guang-Liang, J. Polym. Sci., 19, 3069 (1981). 9 D.W. Sindorf an G. Maciel, J. Am. Chem. Soc., 105, 3767 (1983). 10 E.J.R. SudhSlter, R. Huis, G.R. Hays and N.C.M. Alma, J. Coll. Interf. Sci., 103, 554 (1985). 11 R. Rosset, Bull. Soc. Chim. Fr., 1128 (1985). 12 W.H. Pirkle, T.C. Pochapsky, G.S. Mahler, D.E. Corey, D.S.Reno and D.M. Alessi, J. Org. Chem., 51, 4991 (1986). 13 J.W. De Haan, H.M. Van den Bogaert, J.J. Ponjed and L.J.M. Van de Ven, J. Coll. Interf. Sci., 110, 591 (1986). 14 U. Nagel and E. Kinsel, J. Chem. Soc. Chem. Comm., 1098 (1986). 15 K. Soai, M. Watanabe and A. Yamamoto, J. Org. Chem., 55. 4832 (1990). 16 E.I.S. Adreotti and Y. Gushikem, J. Coll. Interf. Sci., 142, 97 (1991). 17 H.U. Blaser, Tetrahedron Asymmetry, 2, 843 (1991). 18 P. Herman, C. del Pino and E. Ruitz-Hitsky, Chem. Mater., 4, 49 (1992). 19 B. Pugin and M. Miiller, in "Heterogeneous Catalysis and Fine Chemicals III", M.Guisnet et al. Eds., Elsevier Science Publishers, Stud. Surf. Sci. Catal., 78, 107 (1993). 20 Y.G. Akopyants, S.A. Borisenkova, O.L. Kalya, V.M. Derkacheva and E.A. Lukyanets, J. Mol. Catal., 83, 1 (1993). 21 M. McCann, E.M. Giolla and K. Maddock, J. Chem. Soc. Dalton Trans., 1489 (1994). 22 R.S. Drago, J. Gaul, A. Zombeck and D.K. Straub, J. Am. Chem. Soc., 102, 1033 (1980). 23 D.E. De Vos, F. Thibault-Starzyk and P.A. Jacobs, Angew. Chem. Int. Ed. Engl., 33, 431 (1994). 24 S. Brunauer, L.S. Deming, W.S. Deming and E. Teller, J. Am. Chem. Soc., 62, 1723 (1940). 25 A. Cauvel, D. Brunel, F. DiRenzo, P. Moreau and F. Fajula, in Proceeding of Zeocat'95, Stud. Surf. Sci. Catal. in press.
Zeolites: A Refined Tool for Designing Catalytic Sites L. Bonneviotand S. Kaliaguine (editors) 9 1995 Elsevier Science B.V. All rights reserved.
181
Synthesis of mesoporous manganosilicates Mn-MCM-41, Mn-MCM-48 and Mn-MCM-L at a low surfactant/Si ratio Dongyuan Zhao and Daniella Goldfarb Chemical Physics Department, Weizmann Institute of Science, Rehovot, Israel 76100
Mesoporous manganosilicate molecular sieve, Mn-M41 S, having hexagonal (Mn-MCM-41), cubic (Mn-MCM-48), lamellar (Mn-MCM-L) structure, were synthesized in low surfactant/Si ratio (0.12) and characterized by X-ray powder diffraction, transmission electron microscopy (TEM), themogravimetric analysis (TGA) and electron paramagnetic resonance (EPR). The phase transformations trends: hexagonal ~ lamellar ~ cubic -~ hexagonal or hexagonal hexagonal, lamellar mixture ~ cubic ~ lamellar were observed by variations of the base or acid content of the gel or reaction temperature respectively. The results show at low surfactant/Si ratio, Mn-MCM-41 can be synthesized both in acid and base medium, and in a wide range of temperature (21-100~ Mn-MCM-48 can be obtained only in basic medium and in high temperature (100-120~ lamellar phase is formed in high temperature (>130~ and caused the collapse of the structure after calcination at 540~ Addition of Mn ions induces the formation of cubic phase also at low surfactant/Si ratio (0.12). By variations of the base content of the gel, AI-MCM-48 also can be synthesized. EPR results suggest that Mn ions can be incorporated into the amorphous silica wall of M41S or in the interface region of the polar head groups of the template. After calcination, Mn ions in Mn-MCM-41 and Mn-MCM-48, have high mobility and are not located within the inorganic wall.
1. INTRODUCTION Recently a new family of mesoporous molecular sieves designated as M41S was synthesized in the laboratories of the Mobil Oil Company [ 1-3 ]. The M41S materials possess a regular array of uniform mesopores, which can be systematically varied in size from around 20 to 100 A [411 ]. These materials bridge the gap between microporous (zeolites) and macroporous materials (e.g. amorphous aluminosilicates). The members of the M41S family include MCM-41, having a hexagonal arrangement of pores, MCM-48, displaying a cubic structure and other members such as lamellar and cubic octamer, that are not as easily categorized [2-4,6]. The pore size of the M41S materials, their high surface areas (up to 1000 m2g-1), their distinct adsorption properties (pore condensation without hysteresis) [3b], and their thermal stability render them as prim candidates for industrial applications. Modifications in the composition of the silica based M41S materials were so far limited to the incorporation of aluminum, vanadium and titanium into MCM-41 [ 12,15,16]. Similar substitutions have not yet been reported for the silica base cubic phase, MCM-48, which have been
182 synthesized with a high surfactant/Si ratio (1-2) [2,4]. In this work we report on the synthesis of mesoporous manganosilicate materials Mn-M41 S, having hexagonal (Mn-MCM-41), cubic (Mn-MCM-48) and lamellar (Mn-MCM-L) structures, at a low surfactant/silica ratio (0.12), and present a preliminary account on the location of the Mn 2+ cations as obtained from Q-band EPR spectroscopy. We show that the addition of Mn ions induces the formation of the cubic phase also at a low surfactant/Si ratio (0.12) and that by the variation the base content of the gel, one can control the structure formed.
2. EXPERIMENTAL Materials: The synthesis mixture was prepared using sodium silicate, N brand, 27% silica, or tetraethyl orthosilicate (TEOS), Aldrich; Catapal alumina, Condea; Aluminum-isopropylate, Merck; AICI3, Merck; cetyltrimethylammonium chloride (25 wt.%) (CTAC) or bromide (CTAB), Aldrich. Other inorganic materials were MnCI 2 .6H20, Merck, HCI and NaOH. All chemical were used as received. Synthesis: Two Synthesis procedures, differing mainly in the silica source, were employed [2]. In the first, 15-30 ml of 2 M NaOH solution were added under constant stirring to 14.5 ml CTAC or CTAB. The mixture was then combined with 0.1-20 ml of a 0.4 M MnCI 2 solution and 20.5 ml tetraethyl orthosilicate. The composition of the final gel was SiO 2 .xMnO-yNa20 zCTAC(CTAB).wH20 9 , where 0.0004<x<0.09, 0.16
183
Table 1 Synthesis and characterization data of the mesoporous manganese materials Sample
SiO 2
No.
(mmol)
A1CI 3 (mmol)
CTAC CTAB (mmol)
M n 2+ (mmol)
NaOH (HCI) (mmol)
Mn/Si molar ratio
Tem.
product
(~
d-value(A) (first peak)
MCM-41
39.2(32.1) c
MCM-L MCM-48 MCM-48 MCM-41
36.8 39.2(34.6) c 36.0(31.4) c 37.6(30.4) c
100 100 RT
MCM-41 MCM-48 MCM-41
41.3(32o7) c 37.6(31.0) c 39.2(32.1) c
4.3x10 "3 4.3x10 "3
150 100
MCM-L MCM-41
36.0 43.5(33.9) c
0.09 4.3x10 "3 4.3x10 "3 4.3x10 "3 4.3x10 "3
100 100 100 100 100/RT 100
MCM-48 MCM-48 MCM-41 MCM-41 MCM-41 MCM-41
1 2 3 4 5
92 a 61.5 a 52.4 a 92 a 92 b
-
11 11 50.2 11 11
0.4
50 50 55 62 8
4.3x10 "3
RT 150 100 100 100
6 7 8
86 a 92 a 92 a
5 -
11 11 11
0.4 0.4 0.4
55 55 55
4.7x10 "3 4.3x10 "3 4.3x 10 "3
9 10
92 a 92 a
-
11 11
0.4 0.4
55 30
11 12 13 14 15 16
92 a 92 a 92 b 92 b 92 b 92 b
2 -
11 11 11 11 11 11
8.4 0.4 0.4 0.4 0.4
60 65 0 10 d 25 d 41 d
Silica sources: a, tetraethylorthosilicate; b, sodium silicate; c, after calcined at 540~
37.8(32.1) c 37.7(33.2) c 38.4(34.0) c 43.1(40.5) c 45.3(40.0) c 47.7
d, HCI.
3. RESULTS AND DISCUSSION Using the procedures described in the experimental section all three structures, Mn-MCM41, Mn-MCM-48 and Mn-MCM-L could be generated with a wide of Mn/Si molar ratio (0.0004-0.09). Some examples of the materials synthesized, the specific gel compositions, the reaction conditions, the phases obtained and the corresponding d spacings are given in Table I. Typical X-ray diffraction (XRD) patterns of as-synthesized Mn-MCM-41, Mn-MCM-48 and Mn-MCM-L are shown in Fig. 1. Owing to the long range order of the pores they show diffractions in the 20 range of 2-8 ~ similar to XRD patterns previously reported for M41S materials with hexagonal, cubic and lamellar structures [2,5]. Mn-MCM-41 and Mn-MCM-48 are highlystable and their pore structures withstand calcination at 540 o C. The XRD patterns of the calcined materials are similar to those of the as-synthesized materials indicating, how-ever, a reduction in the pore size of--7 A and --5 A in Mn-MCM-41 and Mn-MCM-48 respectively (see Table 1). The BET surface area of calcined Mn-MCM-41 and Mn-MCM-48 was 1340 and 950 mEg-1 respectively, in good agreement with previously reported values [2,3]. Calcination of Mn-MCM-L caused the collapse of the structure as expected [2]. The transmission electron micrograph (TEM) of an as-synthesized Mn-MCM-41 sample, shown in Fig 2a, exhibits a regular array of channels in a hexagonal arrangement [4,7]. The repeat distance between the channels is about 40 A, which is in excellent agreement with the position of the first peak in the XRD pattern (d100=39. 2A, a=2d100/~/3=45.3A) [4,7]. The micrograph also shows that the size of the pores is--30/k with inorganic wall thickness or-~15
184
8vI~ i~
ll
r4)
c
100 36.0 200 17.8
~
211 37.6
421 20.2
II
~n
22o 32.8 332 ,9.r
II
~/V'
32, 2,.5 ,22 ,8.8
I
| 0
~ ,tJ ~
400 23.1
431
18.0 ~
.......
i+i/~
.... , ?
II
A
/I 11
B
1~
/ \ <'' / ~
/tY
\_J,
,1o ,...
' _
39.2
,,o ~2.7 200 ,9.8
M~ I 2
~
I 4
i
I 6
i
I 8
9
l 10
degrees 20
Figure 1. Powder X-ray diffraction patterns of as-synthesizedd Mn-MCM-41, Mn-MCM-48 and Mn-MCM-L.
Figure 2. Transmission electron micrographs of as-synthesized a, Mn-MCM-41 and b, Mn-MCM-48.
A. The frequency and diversity of the fringe patterns obtained from as-synthesized Mn-MCM48, shown in Fig. 2b, suggest the existence of three-dimensional order in more than one projection as expected for an analog of the cubic Ia3d liquid-crystal phase [3b]. This unique pattern is believed to be the [ 111] projection of Mn-MCM-48. Mn-MCM-41 could be produced over a wide range of temperature (21-100~ At room temperature it was detected already after 5 min. of reaction. The hexagonal structure was the first structure observed and we did not detect a precursor lamellar phase at earlier times, as reported by Monnier et al [5] for MCM-41. At a low surfactant/Si ratio, Mn-MCM-48 could be synthesized only at high temperature (100--120~ and the synthesis of pure Mn-MCM-L required either a high temperature (>130~ or a high surfactant/Si ratio. At a fixed gel composition the structure of the Mn-M41S materials obtained depends on the temperature. The XRD patterns of the reaction products as a function of temperature, shown in Fig. 3, exhibit to following order: hexagonal ~ mixture (hexagonal, lamellar) ~ cubic ~ lamellar. Namely, at room temperature pure Mn-MCM-41 was produced and an increase in the temperature transformed it to a lamellar or cubic phase. This indicates that the temperature plays an impor-
185
150~ -
130~ .._
oo t.=_,
120~ ~ _ _ ~ _
100~ 90~ 70~
~.~-
~
50~
~ . . . . ~ ~ 1 ~ 1 ~ 2 4
I~ ~ 6 degrees 29
RT ''
! 8
'
'i
Figure 3. Powder X-ray diffraction patterns of as-synthesized products obtained from the reaction gel (92 mmol TEOS" 11 mmol CTAC 55 mmol NaOH: 0.4 mmol MnCI2:10.6 mol H20 ) as a function of temperature, the reaction time for each sample was 72 hr.
tant role both in terms of template organization and silanol condensation and supports the basic liquid-crystal templating mechanism proposed earlier for M41S materials [2,3,7]. Furthermore, the transformations observed above suggest that the precursor to the M41S structure is a collection of individual silicate surfactant micellar rods. At a fixed temperature and surfactant/Si ratio the structure formed could be controlled by varying the base or acid content of the gel. The structures obtained were, however, a function of the silica source used. When tetraethyl orthosilicate was used, increasing the NaOH concentration while keeping content of all other components constant, resulted in the trend hexagonal ~ lamellar ~ cubic ~ hexagonal (in different samples). In contrast, when sodium silicate was used, the cubic phase was not produced and the order observed with increasing NaOH concentration was hexagonal ~ lamellar. This difference may arise from a faster silicate hydrolysis rates in sodium silicate, resulting in enhanced silanol condensation and the formation of a thicker amorphous silica wall that inhibits the transformation to the cubic phase. In general Mn-MCM-41 could be synthesized under a broader range of conditions as compared to Mn-MCM-48. For example, the base concentration ranges 0.16
186 Table 2 Elemental analyses of the mesoporous manganese materials wt% Sample No. 7 8 9
Sit 2
Mn
42.5 54.9 41.9
0.38 0.24 0.43
C
H
37.5 28.6 41.5
8.60 6.75 9.09
N 2.20 1.74 2.31
Si/Mn molar ratio
C/N molar ratio
N/Si molar ratio
102 210 89
19.9 19.2 21.0
0.22 0.14 0.24
product MCM-48
MCM-41 MCM-L
B
A a
a
C
d
f
Figure 4 Q-band EPR spectra, recorded at A, RT; B, low temperature(150K) of a, assynthesized Mn-MCM-41; b, calcined Mn-MCM-41; c, calcined Mn-MCM-48; d, Mn 2§ impregnated onto MCM-41 materials; e, alter d calcined at 540~ f, 0.1 mM MnCI2 solution in water.
Thermogravimetric analysis (TGA) of Mn-MCM-41, Mn-MCM-48 and Mn-MCM-L in air showed three distinct stages of weight loss at 35-150~ 150-400~ and above 400~ The first stage is due to the desorption of water, the second, which is accompanied by weak exotherms, is due to the combustion and decomposition of organic species (CTAC or CTAB) and the third stage is related to water losses via condensation of silanol groups to form siloxane bonds [7]. The weight loss for Mn-MCM-41, Mn-MCM-48, and Mn-MCM-L is 41.8%, 50.9% and 53% respectively. The composition of these samples as obtained from chemical analysis is given in Table 2. Both the chemical analysis and the TGA data show that at same composition
187 of the gel less template interacts with the inorganic species to form the hexagonal phase as compared to the cubic and lamellar phase. Also, the Mn concentration in the final product was usually similar or higher than in the reaction gel. A better understanding of the role of the Mn ions in determining the structure of the phase formed can be obtained from the location of the Mn ions in the final product. To characterize the Mn ions location we measured X-band and Q-band EPR spectra of the M41S materials before and after calcination. All as-synthesized materials besides those synthesized at RT with HCI did not show any EPR signals either at RT or at 150K. We attribute the absence of the EPR signal to the presence of Mn(IlI) species, rather than Mn(II), since the latter is oxidized to Mn(III) in basic media in air [ 17]. Calcination of these materials, however, did produce a typical spectrum of Mn(II) indicating that during calcination at least part of the Mn(III) was reduced to Mn(II). In contrast, in as-synthesized Mn containing aluminophosphate molecular sieves, which is synthesized under acidic conditions, typical spectra of Mn(II) were readily observed [ 18]. The X-band EPR spectra were poorly resolved due to the presence of forbidden transitions [18], therefore, Q-band spectra were recorded. The Q-band EPR spectrum of Mn-MCM-41 synthesized at RT in the presence of HCI exhibits a typical Mn(II) spectrum with a hyperfine coupling, a, of 81 G and g ~ 2.00, as shown in Fig. 4a. Low intensity forbidden transitions are evident in both the RT and low temperature spectra indicating that the Mn(II) species are rather immobilized at RT [19]. Upon calcination the hyperfine coupling changed to 91 G and the forbidden transitions, still apparent in the low temperature spectrum of the calcined sample, were averaged out in the RT spectrum. This indicates that the Mn(II) species become more mobile after calcination. The same spectrum was obtained from calcined Mn-MCM-41 which did not exhibit Mn(II) EPR signals prior to calcination. The spectrum of calcined Mn-MCM-48, shown in Fig. 4c, is very similar to that of a MnCI 2 solution in 1:1 water/glycerol at both RT and 150K (Fig. 4d) indicating that fully mobile, hydrated Mn 2+ ions are present within the pores. For comparison, samples where MnCI 2 was impregnated onto as-synthesized pure silica MCM-41 were prepared. The spectrum of the as-prepared sample differed significantly from that Mn-MCM-41, whereas that of the calcined impregnated sample was similar to that of calcined Mn-MCM-41. This suggests that in calcined Mn-MCM-41, Mn(II) ions are situated on the surface (internal and external) and not within the silica wall. Moreover, the larger immobility of the Mn(II) species in the as-synthesized Mn-MCM-41 can be attribute either to its location within the wall or in the interface region of the polar head groups the template and the silica walls. In the calcined samples of both Mn-MCM-41 and Mn-MCM-48, however, their high mobility provides further evidence that they are not located within the inorganic wall.
4. CONCLUSIONS Mesoporous manganosilicate, Mn-M41S, materials with a having hexagonal, cubic and lamellar structures, were synthesized at a low surfactant/Si ratio (0.12). For a fixed gel composition the phase formed could be controlled by the reaction temperature and at a constant temperature, the phase generated was dependent on the NaOH content. The addition of Mn ions induced the formation of cubic phase also at a low surfactant/Si ratio. Prior to calcination the Mn 2+ ions in Mn-MCM-41 are highly immobilized whereas in calcined Mn-MCM-41 and Mn-MCM-48, the Mn 2§ ions are hydrated and highly mobile located within the pore and not in the inorganic wall.
188 5. ACKNOWLEDGMENT We thank Dr. Lev Margulis for performing the TEM measurements.
REFERENCES
1. C.T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710. 2. J.S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T.-W. Chu, D. H. Olson, E. W. Shepard, S. B. McCullen, J. B. Higgins and J. L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. 3. (a) J. S. Beck, J. C. Vartuli, G. J. Kennedy, C. T. Kresge, W. J. Roth and S. E. Schranm, Chem. Mater., 6 (1994) 1861. (b) J. C. Vartuli, K. D. Schmitt, C. T. Kresge, W. J. Roth, M. E. Lenowicz, S. B. McCullen, S. D. Hellring, J. S. Beck, J. L. Schlenker, D. H. Olson and E. W. Sheppard, Chem. Mater., 6 (1994)2317. (c)J. C. Vartuli, C. T. Kresge, M. E. Leonowicz, A. S. Chu, S. B. McCullen, I.