Studies in Surface Science and Catalysis 141 NANOPOROUS MATERIALS III
This Page Intentionally Left Blank
Studies
in S u r f a c e
A d v i s o r y Editors:
Science
and Catalysis
B. Delmon and J.T. Yates
Vol. 141
NANOPOROUS
MATERIALS !11
Proceedings of the 3 '~ International Symposium on Nanoporous Materials, Ottawa, Ontario, Canada, June 12-15, 2002
Edited by A. Sayari
University of Ottawa, Department of Chemistry, Ottawa, Ontario K1N 6N5, Canada
M. Jaroniec
Kent State University, Department of Chemistry, Kent, Ohio 44242, USA
-
¢
2002
ELSEVIER
A m s t e r d a m - Boston - London - New Y o r k - Oxford - Paris - San Diego San Francisco - Singapore - S y d n e y - Tokyo
ELSEVIER SCIENCE B.V. Sara Burgerhartstraat 25 P.O. Box 211, I000 AE Amsterdam, The Netherlands
© 2002 Elsevier Science B.V. All rights reserved.
This work is protected under copyright by Elsevier Science, and the following terms and conditions apply to its use: Photocopying Single photocopies of single chapters may be made for personal use as allowed by national copyright laws. Permission of the Publisher and payment of a fee is required for all other photocopying, including multiple or systematic copying, copying for advertising or promotional purposes, resale, and all forms of document delivery. Special rates are available for educational institutions that wish to make photocopies for non-profit educational classroom use. Permissions may be sought directly from Elsevier Science Global Rights Department, PO Box 800, Oxford OX5 1DX, UK; phone: (+44) 1865 843830, fax: (+44) 1865 853333, e-mail:
[email protected]. You may also contact Global Rights directly through Elsevier's home page (http://www.elsevier.com), by selecting 'Obtaining Permissions'. In the USA, users may clear permissions and make payments through the Copyright Clearance Center, Inc., 222 Rosewood Drive, Danvers, MA 01923, USA; phone: (+1) (978) 7508400, fax: (+1) (978) 7504744, and in the UK through the Copyright Licensing Agency Rapid Clearance Service (CLARCS), 90 Tottenham Court Road, London WIP 0LP, UK; phone: (+44) 207 631 5555; fax: (+44) 207 631 5500. Other countries may have a local reprographie rights agency for payments. Derivative Works Tables of contents may be reproduced for internal circulation, but permission of Elsevier Science is required for external resale or distribution of such material. Permission of the Publisher is required for all other derivative works, including compilations and translations. Electronic Storage or Usage Permission of the Publisher is required to store or use electronically any material contained in this work, including any chapter or part of a chapter. Except as outlined above, no part of this work may be reproduced, stored in a retrieval system or transmitted in any form or by any means, electronic, mechanical, photocopying, recording or otherwise, without prior written permission of the Publisher. Address permissions requests to: Elsevier Science Global Rights Department, at the mail, fax and e-mail addresses noted above. Notice No responsibility is assumed by the Publisher for any injury and/or damage to persons or property as a matter of products liability, negligence or otherwise, or from any use or operation of any methods, products, instructions or ideas contained in the material herein. Because of rapid advances in the medical sciences, in particular, independent verification of diagnoses and drug dosages should be made.
First edition 2002 Library of Congress Cataloging in Publication Data A catalog record from the Library of Congress has been applied for.
British Library Cataloguing in Publication Data A catalogue record from the British Library has been applied for.
ISBN: ISSN:
0-444-51113-X 0167-2991
The paper used in this publication meets the requirements of ANSI/NISO Z39.48-1992 (Permanence of Paper). Printed in The Netherlands.
PREFACE Since the Breck Award winning discovery of the so-called M41S silica mesostructures in the early nineties, the field of ordered mesoporous materials has grown so dramatic that it has developed into a distinct research area. Remarkably, in the last ten years, over 3000 papers have been published on such materials. Impressive progress has been achieved in the use of self-assembly approaches and supramolecular templating techniques to generate a Wide variety of ordered inorganic, organic and hybrid mesostructures with tailored framework composition, pore structure, pore size, morphology and surface properties. The range, of synthesis conditions and the variety of templating surfactants and oligomers that have been explored is truly remarkable. Many fascinating discoveries have been made not only in the rational design of such materials at the molecular level, but also in a wide range of potential applications, for example in adsorption, catalysis, separation processes, environmental cleanups and optoelectronics. Among the most recent developments in this area is the extension of the amphiphile selfassembly techniques to the synthesis of ordered mesoporous organosilicas, which demonstrated that there are almost unlimited opportunities in tailoring surface and structural properties of mesoporous materials. Another important discovery is the use of ordered nanoporous silica and colloidal crystals to create new periodic mesoporous and macroporous materials, including carbons, polymers, metals, and alloys. Combination of different synthesis approaches such as amphiphile, colloidal crystal or microemulsion templating, micromolding and soft lithography led to materials with hierarchically ordered structures. International Symposia on Nanoporous Materials are intended to bring together investigators to discuss complementary approaches and recent advances concerning not only materials synthesized through supramolecular templating, but also a variety of other nanoporous materials such as clays, carbon molecular sieves, porous polymers, sol-gel and imprinted materials as well as self-assembled organic and organometallic zeolite-like materials. Judging from the remarkable success of the previous symposium "Nanoporous Materials II" (May 2000, Banff, Canada), and from the wide range of high quality abstracts and manuscripts submitted to the current meeting, the Organizing Committee is confident that the Nanoporous Materials III symposium will achieve its objective of gathering scientists interested in sharing their valuable findings related to a large variety of nanoporous materials. The contents of the current volume presents a sampling of more than 160 oral and poster papers that will be presented at the Symposium on Nanoporous Materials III held in Ottawa, Canada on June 12-15, 2002. The selected papers cover the three main themes of the symposium: (i) synthesis of mesoporous silicas and related materials (ii) synthesis of other nanoporous and nanostructured materials, and (iii) characterization and applications of nanoporous materials. Compared to the proceedings of the previous symposium, the current volume contains more contributions related to catalytic and environmental applications, which is a very positive trend. Although the present book does not cover all topics in the area of nanoporous materials, it reflects the current trends and advances in this field, which will certainly continue to attract the attention of materials scientists around the globe. Finally, on behalf of the Organizing Committee, we gratefully acknowledge the generous support of the Faculty of Science (University of Ottawa), the National Research Council of Canada (NRC), the Steacie Institute for Molecular Sciences (SIMS) and the University of Ottawa's Centre for Catalysis Research and Innovation (CCRI). Abdel Sayari February 18, 2002 Mietek Jaroniec
This Page Intentionally Left Blank
vii
ORGANIZING COMMITTEE Chairman
Abdel Sayari
University of Ottawa, Ottawa, Ontario, Canada
Vice-Chairman
Mietek Jaroniec
Kent State University, Ohio, USA
Members
Markus Antonietti JeffBrinker Christian Detellier Kazuyuki Kuroda John Ripmeester
Max-Planck-Institute of Colloids and Interfaces, Germany University of New Mexico, New Mexico, USA University of Ottawa, Ottawa, Ontario, Canada Waseda University, Tokyo, Japan National Research Council, Ottawa, Canada
INTERNATIONAL ADVISORY COMMITTEE D. Antonelli G. Attard A. Cheetham J.H. Clark C. Crudden E. Derouane M. Fr6ba A. Galameau S. Inagaki K. Kaneko S. Komameni M. Kruk R. Kumar B. Lebeau Th. Maschmeyer C.Y. Mou G. Q. Max Lu A. Neimark E. Prouzet H.-K. Rhee W.J. Roth D.M. Ruthven R. Ryoo F. Schtith A. Stein M. St6cker B.-L. Su T. Tatsumi O. Yaghi M. Ziolek
University of Windsor, Ontario, Canada University of Southampton, United Kingdom University of California, Santa Barbara, Califomia, USA University of York, York, England University of New Brunswick, NB, Canada University of Liverpool, United Kingdom Justus-Liebig-University, Giessen, Germany Ecole Nationale' Sup6rieure de Chimie de Montpellier, France Toyota Central R&D Laboratories, Inc., Nagakute, Japan Chiba University, Chiba, Japan Pennsylvania State University, University Park, PA, USA Kent State University, Ohio, USA National Chemical Laboratory, Pune, India Universit6 de Haute Alsace, Mulhouse, France Delft University of Technology, The Netherlands National Taiwan University, Taipei, Taiwan The University of Queensland, Brisbane, Australia TRI/Princeton, New Jersey, USA Ecole Nationale Sup6rieure de Chimie de Montpellier, France Seoul National University, Seoul, Korea Exxon-Mobil Research and Engineering Co., New Jersey, USA University of Maine, Orono, Maine, USA KAIST, Taejon, Korea MPI ftir Kohlenforschung, Mtilheim, Germany University of Minnesota, Minneapolis, Minnesota, USA SINTEF, Oslo, Norway The University of Namur, Belgium Yokohama National University, Yokohama, Japan University of Michigan, Ann Arbor, Michigan, USA A. Mickiewicz University, Poznan, Poland
This Page Intentionally Left Blank
ix
CONTENTS
Preface Organizing Committee
vii
Intemational Advisory Committee
vii
I.
Plenary Lectures
Recent Developments in the Synthesis and Chemistry of Periodic Mesoporous Organosilicas Tewodros Asefa, Geoffrey A. Ozin, Hiltrud Grondey, Michal Kruk, and Mietek Jaroniec Porous Materials: Looking Through the Electron Microscope O. Terasaki, T. Ohsuna, Z. Liu, M. Kaneda, S. Kamiya, A. Carlsson, T. Tsubakiyama, Y. Sakamoto, S. Inagaki, S. Che, T. Tatsumi, M. A. Camblor, R. Ryoo, D. Zhao, G. Stucky, D. Shindo and K. Hiraga
27
Molecular Imprinting - A Way to Prepare Effective Mimics of Natural Antibodies and Enzymes Giinter Wulff
35
II. Synthesis of Mesoporous Silicas Plugged Hexagonal Mesoporous Templated Silica: A Unique Micro- and Mesoporous Material with Internal Silica Nanocapsules P. Van Der Voort, P. I. Ravikovitch, A. V. Neimark, M. Benjelloun, E. Van Bavel, K.P. De Jong, B. M. Weckhuysen and E.F. Vansant
45
Imprinting of the Surface of Mesoporous Silicates using Organic Structure Directing Agents Kaveri R. Sawant and Raul F. Lobo
53
Synthesis and Characterization of Polymer-Templated Ordered Silica with Cagelike Mesostructure J.R. Matos, M. Kruk, L.P. Mercuri and M. Jaroniec
61
The Modeling of Wall Structure of Siliceous MCM-41 Based on the Formation Process Yasunori Oumi, Kazuhiko Azuma, Takuji Ikeda, Shintaro Sasaki and Tsuneji Sano
69
Pore Size Adjustment of Bimodal-mesoporous Silica Molecular Sieves Xiaozhong Wang, Tao Dou, Dong Wu and Bing Zhong
77
Alcothermal Synthesis of Large Pore, High Quality MCM-48 Silica Jihong Sun and Marc-Olivier Coppens
85
Studies of MCM-41 Obtained from Different Sources of Silica Icaro S. Paulino and Ulf Schuchardt
93
Synthesis and Characterization of Hexagonal Mesoporous Materials Using Hydrothermal Restructuring Method Kyoung-Ku Kang and Hyun-Ku Rhee
101
Synthesis of Highly Ordered Mesoporous Compounds with Control of Morphology Using a Non-ionic Surfactant as Template A. LOonard, J.L. Blin and B. L. Su
109
Towards a Better Understanding on the Mechanism of Mesoporous Formation via an Assembly of Cn(EO)mTMOS J.L. Blin, A. L~onard, G. Herrier, G. Philippin and B.L. Su
117
Mesoporous Silicas via Organic-Inorganic Hybrids Based on Charged Polymers Graham M. Gray and John N. Hay
127
Mesoporous Silicas of Hierarchical Structure by Hydrothermal SurfactantTemplating under Mild Alkaline Conditions Zhong-Yong Yuan, Wuzong Zhou, Bao-Lian Su and Lian-Mao Peng
133
III. Synthesis of Framework-Modified Mesoporous Silicas Synthesis and Characterisation of Super-microporous Aluminosilicates Prepared via Primary Amine Templating E. Bastardo-Gonzalez, Robert Mokaya and William Jones
141
A1-MCM-41 Synthesis Studies Using Al-Isopropoxide as A1 Source R. Birjega, R. Ganea, C. Nenu, Gr. Pop, A. Jitianu
.151
Mesoporous Aluminosilicates from Coal Fly Ash P. Kumar, N. Mal, Y. OumL T. Sano and K. Yamana
159
xi New Route for Synthesis of Highly Ordered Mesop0rous Silica with Very High Titanium Content Xiang-Hai Tang, Xin Wen, Shi-Wei Sun and Hai-Yan Jiang
167
Synthesis and Characterization of Ti-containing Mesoporous Alumina Molecular Sieves Chun Yang and Xi Li
173
IV. Synthesis of Surface-Modified Mesoporous Silicas Organizing One-Dimensional Molecular Wires in Ordered Mesoporous Silica Zongtao Zhang, Douglas A. Blom and Sheng Dai
183
Synthesis and Catalytic Properties of Organically Modified Ti-HMS Yong Yang and Abdelhamid Sayari
189
Synthesis and Characterization of Methyl- and Vinyl-Functionalized Ordered Mesoporous Silicas with High Organic Content Michal Kruk, Tewodros Asefa, Mietek Jaroniec and Geoffrey A. Ozin
197
Polyfunctionalized Silica Adsorbents Obtained by Using Dodecylamine as Template Inna V. Mel'nyk (Seredyuk), Yuriy L. Zub, Alexey A. Chuiko, Mietek Jaroniec and Stephan Mann
205
Characterization of Mesoporous Thin Films Formed with Added Organophosphonate and Organosilane Michael A. Markowitz, Eva M. Wong and Bruce P. Gaber
213
Improving the Hydro-Stability ofMCM-41 by Post-Synthesis Treatment and Hexamethyldisilazane Coating Jing Yang, Antje Daehler, Michelle L. Gee, Geoffrey W. Stevens and Andrea J. O'Connor
221
Adsorption of CO on Zn-Cu(I)/HMCM-41 Qihong Shi, Nongyue He, Fei Gao, Yibing Song, Yang Yu and Huilin Wan
229
V.
Synthesis of Mesoporous Metal Oxides
Design of Transition Metal Oxide Mesoporous Thin Films Eduardo L. Crepaldi, Galo J. de A. A. Soler-Illia, David Grosso, PierreAntoine Albouy, Heinz Amenitsch and ClOment Sanchez
235
xii Mesoporous Alumina as A Support for Hydrodesulphurization Catalysts Jiri Cejka, Nadezda Zilkovd, Ludgk Kalu$a and Miroslav Zdra~il
243
Preparation and XAFS Spectroscopic Characterization of Mesoporous Titania with Surface Area more than 1200 m2/g Hideaki Yoshitake, Tae Sugihara and Takashi Tatsumi
251
Mesoporous Zirconium Oxides: An Investigation of Physico-chemical Synthesis Parameters J.L. Blin, L. Gigot, A. L~onard and B.L. Su
257
Single Crystal Particles ofMesoporous (Nb, Ta)205 Junko N. Kondo, Tomohiro Yamashita, Tokumitsu Katou, Byongjin Lee, Daling Lu, Michikazu Hara and Kazunari Domen
265
VI. Synthesis of Other Nanostructured Materials and Nanoparticles Preparation of Exfoliated Zeolites from Layered Precursors - The Role of pH and Nature of Intercalating Media Wieslaw J. Roth and James C. Vartuli
273
Control of Mesopore Structure of Smectite-type Materials Synthesized with a Hydrothermal Method Masayuki Shirai, Kuriko Aoki, Kazuo Torii and Masahiko Arai
281
Synthesis, Characterization and Catalytic Application of Mesoporous Sulfated Zirconia Young-Woong Suh and Hyun-Ku Rhee
289
Synthesis of Mesoporous Silicoaluminophosphates (SAPO) Erica C. de Oliveira and Heloise O. Pastore
297
Synthesis and Characterization of Mesostructured Vanadium-Phosphorus-Oxide Phases Moises A. Carreon and Vadim V. Guliants
301
Novel Macroporous Vanadium-Phosphorus-Oxides Arrays of Spherical Voids Moises A. Carreon and Vadim V. Guliants
309
with Three-Dimensional
Engineering Active Sites in Bifunctional Nanopore and Bimetallic Nanoparticle Catalysts for One-Step, Solvent-Free Processes Robert Raja and John Meurig Thomas
317
xiii Using Au Nanoparticles-Surfactant Aqueous Solution for a Convenient Preparation of Mesoporous Aluminosilicates Containing Au-Nanoparticles Yu-Shan Chi, Hong-Ping Lin, Chinn-Nan Lin, Chung-Yuan Mou and BenZu Wan
329
The Use ofTemplated Mesoporous Materials as Tempates for the Development of Odered Arragements of Nanowire and Nanorods of Electronically Important Materials J. D. Holmes, T. R. Spalding, K. M. Ryan, D. Lyons, T. Crowley and M. A. Morris
337
Synthesis and Adsorption Properties of Novel Carbons of Tailored Porosity Z. Li, M. Kruk and M. Jaroniec
345
Flexible Metal-Organic Frameworks with Isomerizing Building Units D. V. Soldatov and J. A. Ripmeester
353
Dynamic Porous Frameworks of Coordination Polymers Controlled by Anions Shin-ichiro Noro and Susumu Kitawaga
363
Mesoporous Polymeric Materials Based On Comb-Coil Supramolecules Sami Valkama, Riikka Miiki-Ontto, Manfred Stamm, Gerrit ten Brinke and Olli Ikkala
371
VII.
Characterization of Nanoporous Materials
Electron Microscopic Investigation of Mesoporous SBA-2 Wuzong Zhou, Alfonso E. Garcia-Bennett, Hazel M. A. Hunter and Paul A. Wright
379
A Study of Morphology of Mesoporous Silica SBA-15 Man-Chien Chao, Hong-Ping Lin, Hwo-Shuenn Sheu and Chung-Yuan Mou
387
SBA- 15 versus MCM-41: Are they the same Materials? Anne Galarneau, HOlOne Cambon, Thierry Martin, Louis-Charles De M~norval, Daniel Brunel, Francesco Di Renzo and Franfois Fajula
395
Comprehensive Characterization of Iron Oxide Containing Mesoporous Molecular Sieve MCM-41 Zhong-Yong Yuan, Wuzong Zhou, Zhaoli L. Zhang, Q. Chen, B.L. Su, and Lian-Mao Peng
403
xiv Mesoporous Molecular Sieves of MCM-41 Type Modified with Cs, K and Mg Physico-Chemical and Catalytic Properties Maria Ziolek, Aleksandra Michalska, Jolanta Kujawa and Anna Lewandowska
411
Meso-ALPO Prepared by Thermal Decomposition of the Organic-Inorganic Composite. A FTIR Study Enrica GianottL Erica C. Oliveira, Valeria Dellarocca, Salvatore Coluccia, Heloise O. Pastore and Leonardo Marchese
417
Organic - Inorganic Phase Interaction in A1SBA-15 Mesoporous Molecular Sieves by Double Resonance NMR Spectroscopy Jean-Baptiste d'Espinose, Elias Haddad and Antoine G~dOon
423
Adsorption of Nitrogen on Organized Mesoporous Alumina Jiri Cejka, Lenka Vesel6, Jiri Rathousk~ and Arnogt Zukal
429
The Use of Ordered Mesoporous Materials for Improving the Mesopore Size Analysis: Current State and Future Michal Kruk, Mietek Jaroniec and Abdelhamid Sayari
437
Sorption Properties and Hydrothermal Stability of MCM-41 Prepared by pH Adjustment and Salt Addition Nawal Kishor Mal, Prashant Kumar and Masahiro Fujiwara
445
Acidity Characterization ofMCM-41 Materials Using Solid-State NMR Spectroscopy Qi Zhao, Wen-Hua Chen, Shing-Jong Huang, Yu-Chih Wu, Huang-Kuei Lee and Shang-Bin Liu
453
Acidity of Calcined AI-, Fe-, and La-containing MCM-41 Mesoporous Materials: An Investigation of Adsorption of Pyridine Nong-Yue He, Chun Yang and Zu-Hong Lu
459
Acid Properties of Ammonium Exchanged A1MCM-41 with Different Si/A1 Ratio Antonio S. Arafijo, Cristiane D.R. Souza, Marcelo J.B. Souza, Valter J. Fernandes Jr., and Luiz A. M. Pontes
467
Kinetic Evaluation of the Pyrolysis of High Density Polyethylene over HA1MCM-41 Material Antonio S. Arafijo, Valter J. Fernandes Jr, Sulene A. Araujo and Massao Ionashiro
473
Electrorheological Response of Mesoporous Materials under Applied Electric Fields Min S. Cho, Hyoung J. Choi, Wha-Seung Ahn and Myung S. Jhon
479
XV
VIII. Catalytic Applications of Nanoporous Materials Synthesis and Characterization of TiO2 Loaded Cr-MCM-41 catalysts E.P. Reddy, Lev Davydov and Panagiotis G. Smirniotis
487
Photocatalytic Ethylene Polymerization over Chromium Containing Mesoporous Molecular Sieves Hiromi Yamashita, Katsuhiro Yoshizawa, Masao Ariyuki, Shinya Higashimoto and Masakazu Anpo
495
Catalytic Reduction of Nitric Oxides on A1- containing Mesoporous Molecular Sieves W. Li, Y. Zhang, Y. Lin and X. Yang
503
Catalytic Oxidation of alpha-Eicosanol to alpha-Eicosanoic Acid Over Ti, Zr and Mn Doped MCM-48 Molecular Sieves Changping Wei, Yining Huang, Qiang CaL Wenqin Pang, Yingli BL and Kaiji Zhen
511
Preparation of Pd/A1-MCM-41 Catalyst and Its Hydroisomerization Properties for Long Chain Alkane Compounds Shui Lin, Han Ning, Sun Wan-Fu, Liu Wei-Min and Xue Qun-Ji
517
Alkylation of Phenol with Methyl tert-Butyl Ether over Mesoporous Material Catalysts Xiang-Hai Tang, Xin-Liang Fu and Hai-Yan Jiang
525
Isopropanol Dehydration over Nanostructured Sulfated MCM-41 Antonio S. Araujo, Joana M.F.B. Aquino, Cristiane D.R. Souza and Marcelo J.B. Souza
531
Effect of Si/A1 Ratio and Pore Size on Cracking Reaction over Mesoporous MCM-41 Wen-Hua Chen, Qi Zhao, Hong-Ping Lin, Chung-Yuan Mou and ShangBin Liu
537
Hydrogenation and Mild Hydrocracking of Synthetic Crude Distillate by Ptsupported Mesoporous Material Catalysts Hong Yang, Craig Fairbridge, Zbigniew Ring, Randall Hawkins and Josephine M. Hill
543
Carbon-Carbon Bond Forming Reactions Catalyzed by Meso- and Microporous Silicate-Quaternary Ammonium Composite Yoshihiro Kubota, Yusuke Nishizaki, Hisanori Ikeya, Junko Nagaya and Yoshihiro Sugi
553
xvi A Selectivity of Zeolite Matrices in the Cu(II) Reduction Process Vitalii PetranovskiL Valerij Gurin, Nina Bogdanchikova, Miguel-Angel Hernandes and Miguel A valos
561
Reduction of Binary Silver-Copper Ion Mixture in Mordenite: an Example of Synergetic Behavior Vitalii Petranovskii and Nina Bogdanchikova
569
Preparation, Characterization and Catalytic Properties of CuPC/Y Nanocomposite Huaixin Yang, Ruifeng Li and Kechang Xie
575
IX.
Environmental Applications of Nanoporous Materials
Environmental Applications of Self-Assembled Monolayers on Mesoporous Supports (SAMMS) Glen E. Fryxell, Yuehe Lin, Hong Wu and Kenneth Kemner
583
A Possible Use of Modified Mesoporous Molecular Sieves in Water Treatment Processes Izabela Nowak, Barabara Kasprzyk, Maria Ziolek and Jacek Nawrocki
591
Organized Mesoporous Titanium Dioxide - A Powerful Photocatalyst for the Removal of Water Pollutants Jiri Rathouslc~, Mark~ta Slabovd, Katerina Macounovd and Arnogt Zukal
599
Mesoporous Materials for Heavy Metal Ion Adsorption Synthesized by Displacement of Polymeric Template V. Antochshuk, M. Jaroniec, S.H. Joo and R. Ryoo
607
Organically-modified Mesoporous Silica Spheres with MCM-41 Architecture as Sorbents for Heavy Metals M. Etienne, S. Sayen, B. Lebeau, and A. Walcarius
615
NO and NO2 Gas Sensors Based on Surface Photovoltage System are Fabricated by Self-ordered Mesoporous Silicate Film Hao-Shen Zhou, Takeo Yamada, Keisuke Asai, Itaru Honma, Hidekazu Uchida and Teruaki Katsube
623
xvii
XO
Other Applications of Nanoporous Materials
Polymerisations in Mesoporous Environments James H. Clark, Duncan Macquarrie, Valerie Sage, Katie Shorrock and Karen Wilson
631
Incorporation ofNano-sized zeolites into a Mesoporous Matrix, TUD-1 Z. Shah, W. Zhou, J.C. Jansen, C. Y. Yeh, J.H. Koegler and Th. Maschmeyer
635
Formation and Stabilization of Gold Nanoparticles in Organo-Functionalized MCM-41 Mesoporous Materials and their Catalytic Applications Chitta Ranjan Patra, Anirban Ghosh, Priyabrata Mukherjee, Murali Sastry and Rajiv Kumar
641
Entrapment and Stabilization of Cadmium Sulphide (CdS) Nanoclusters Formed Inside Propylthiol Functionalized MCM-41 Mesoporous Materials Anirban Ghosh, Chitta Ranjan Patra, Priyabrata Mukherjee, Murali Sastry and Rajiv Kumar
647
SnO2 Nanoparticles in the Pores of Non-structured SiO2 and of Si-MCM-41: Comparison of their Properties in Gas Sensing Yuecel Altindag, Andrei Jitianu and Michael Wark
653
Spontaneous Nitride Formation in the Reaction of Mesoporous Titanium Oxide with Bis(Toluene) Titanium in a Nitrogen Atmosphere. M. Vettraino, X. He, Michel Trudeau and David Antonelli
661
Isolation and Characterization of Amorphous Solids from Oil Sands Fine Tailings Abdul Majid, Steve Argue, Irina Kargina, Victor Boyko, Gerry Pleizier and Jim Tunney
669
Author Index
675
Subject Index
679
This Page Intentionally Left Blank
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
Recent developments in the synthesis and chemistry o f periodic m e s o p o r o u s organosilicas
9
a*
Tewodros Asefa, a Geoffrey A. Ozln, ' Hiltrud Grondey, a Michal Jaroniec b
KIRlk, b
and Mietek
a Materials
Chemistry Research Group, Department of Chemistry, University of Toronto, Toronto, Ontario M5S 3H6, Canada b Department of Chemistry, Kent State University, Kent, Ohio 44242, USA
Synthetic routes have recently been developed to an entirely new class of organicinorganic hybrid nanocomposite materials called periodic mesoporous organosilicas (PMOs) containing bridging organic groups integrated within a well-ordered mesoporous silica-based framework structure. Some of the interesting properties of these types of materials have been demonstrated but real challenges still remain including the scope of the synthesis approach and breadth of the compositional domain, reactivity and stability of the materials, their chemical and physical, electrical and mechanical properties, as well as potential applications. In this review, we will describe our past and current research concerning new synthetic strategies, unique properties and advantageous features of alkane, alkylene, aromatic, heteroatom-containing, chiral, and star-like organic functional group containing PMOs as advanced materials for diverse applications. Some of the effects of size and kind of organic groups on the order and integrity of the structure of the materials are discussed. Various synthetic routes, such as lithiation, Grignard, hydroboration, Pd-catalysed Heck coupling and alcoholysis reactions that we used to make the molecular poly(trialkoxysilyl)organic precursors are also briefly described.
I. INTRODUCTION The synthesis of periodic mesoporous organosilica (PMO) materials containing organic groups in the framework of ordered and high surface area mesostructures is drawing increasing attention recently [1-30]. One of the main driving forces behind the synthesis of various PMOs is the traditional interest in the synthesis of ordered hybrid organic-inorganic nanocomposites wherein beneficial properties of one of the components are enhanced or new properties uncharacteristic of the individual components are created. Furthermore, the presence of organic functional groups in such ordered nanoporous materials also offers additional advantages that make the materials potentially useful as catalytic and chromatographic supports, chemical and biological
sensors and membranes. Consequently, research in the field of organic-inorganic hybrid nanocomposite materials has remained an active area of investigation for the last few decades and is likely to expand in the years as well. Enormous advances made since the first types of classical organically modified silicas (ORMOSILs) and organically modified ceramics (ORMOCERS) were reported [31-33]. The successes in coupling organic and inorganic groups at a molecular level for the synthesis of hybrid organicinorganic xerogels and amorphous materials [34-40] have also led to many advances in recent years and proved to have advantages over thesimple physical mixing of the constituents in their bulk states. However, until recently, there have been no welldeveloped approaches to create uniform pores of controlled size in these materials. In fact, their porous structure is highly dependent on the synthesis temperature and drying conditions [39,40]. With the work of Mobil scientists in 1992 and the first report on mesoporous silica (MCM-41) materials [41-44], a new research direction in organicinorganic nanocomposite materials emerged. The synthesis of these materials is carried out using inorganic precursors and surfactant templates and the method of supramolecular self-assembly. In many cases, the supramolecular templates can be removed without the collapse of the ordered composite, thus rendering ordered mesoporous structures. After the first papers on materials with siliceous frameworks [41-44], synthesis techniques and compositions of mesoporous materials developed further to include various other kinds of nanocomposite and nanoporous materials. The methodology, for instance, was modified to include ordered hexagonal, cubic and lamellar structures as well as disordered structures with uniform pores [41-50] while the composition field was expanded to include Pt, TiO2, M/Ge4Sl0, etc. [51-57]. Furthermore, by judicial choice of templates and swelling agents, control over the size, porosity and structure of the materials have been achieved [41,49,50,58,59]. The literature in the past 10 years also contains demonstrations on potential applications of these materials in catalysis, nanoelectronics, separation, host-guest chemistry and sensing [60-66]. However, many of these applications were not achieved with the periodic structure alone. The presence of electroactive, optically active or reactive functional sites within these high surface area and ordered mesoporous materials were required for these applications to be realized in practice. The introduction of terminal organic functional groups into periodic mesoporous silicas either through direct or indirect (post-synthetic) synthetic approaches has been successfully used as a way to functionalize this class of materials in the past few years [67-71 ]. However, these approaches have often resulted in materials with lower degree of structural ordering and low or moderate loading of organic groups. The recent approach of introducing organic functional groups into the framework of periodic mesoporous organosilicas (PMO) provided a way to overcome these drawbacks [ 1-30]. PMOs are a new class of organic-inorganic hybrid nanocomposites with uniformly distributed organic functional groups in the framework of the materials. They are synthesized like MCM-41 materials through in a one-pot surfactant-templated supramolecular self-assembly procedure but from the hydrolysis and condensation of poly(trialkoxysilyl)organic precursors ([(R'O)3Si]xR, x = 2 ,3) [1-30]. The enormous choice of polysilylated molecular precursors having various types of bridging organic functional groups with for example electroptic, catalytic and hydrophilic/hydrophobic
properties and the self assembly of these with various kinds of supermolecular templates are providing researchers with large varieties of periodic mono- and multi-functional organic-inorganic nanocomposite materials. The ability for molecular integration of organic and inorganic groups in the framework of these materials may have advantages over direct and indirect (grafting)methods that may create non-uniformly distributed organic groups protruding into the void spaces. Benefits include tailorable physical properties [ 19,20], uniform distribution of functional groups, possibility of controlling the loading of the functional groups using co-condensation approach, and unique chemical properties. Some of these bridging organic groups have also proven to be accessible for chemistry and can be further transformed chemically [1,18]. Interesting chemical differences between organics in the framework and in the channels has been reported and used to have advantages in the preparation of a new sub-class of bifunctional and multifunctional PMOs [8]. The dependence of thermal, mechanical, dielectric and adsorptions properties on the nature of the organic groups in these hybrid materials will likely result in new products, processes and devices made out of PMOs in the near future [3,19-21 ]. The ability to synthesize film and various curved PMO morphologies [7,19-21] may lead to advances in catalysis, chromatography and membrane science and technology. Advances made in the synthesis and characterization of the properties of PMO materials in just less than two years have inspired investigations into new kinds of functionalized PMO materials and a search for commercial applications. However, only a few types of organic functionalized PMOs have been reported so far. They include methylene, ethane, ethylene, acetylene, thiophene, benzene and bithiophene containing PMOs, [ 1-30]. There is also a notable scarcity of detailed investigations of the structural integrity, and thermal and chemical stability of Si-C bonds for various kinds of organic groups in PMOs [3,8]. Herein, we review some developments in our research group mainly concerning the synthesis of various PMO materials and possible applications. Particular attention will be given to PMO materials having heteroatom and side-arm starlike organic groups, which are envisioned to enhance the reactivity and accessibility of bridging organic groups in PMOs enabling judicious surface modification that leads to the tailoring of function. 2. E X P E R I M E N T A L 2.1. Materials. HC1 and NH 3 solutions were obtained from BDH. Methanol was supplied by ACP. Hexanes, pentanes, diethylether and tetrahydrofuran (THF) were purchased from ACP and were dried with Call2 and molecular sieves before every use. The THF and the diethylether were further distilled over Na/benzophenone. All commercially available bis(triethoxysilyl)organic compounds were obtained from Gelest. All other chemicals were received from Aldrich. 2.2. PMO PRECURSORS 2.2.1. Commercially available PMO precursors. Scheme 1 shows most of the commercially available precursors (either triethoxysilylated or trichlorosilylated) that we
obtained from Gelest and used for the preparation of PMOs. The precursors were used as received without further purification.
Scheme 1. Commercially available PMO precursors used for the synthesis of PMO materials (Si denotes -Si(OEt)3 or-SIC13).
Si~Si
Si~si
1
Si~"x,~"X, Si
2
3
4
~---Si S
~
S i ~ S i
S i ~ N H
Si Si 6
S i ~ N H 7
2.2.2. Synthesis of PMO precursors.
We have utilized various synthetic routes to prepare polyalkoxysilylated PMO precursors that are not commercially available. Representative synthetic routes are shown in Scheme 2 and some examples of PMO precursors and PMOs that we have prepared from these precursors are shown in Scheme 3. Some of these precursors have been synthesized before and used to prepare hybrid org~ic-inorganic xerogels (materials with a relatively broad pore size distribution) by many groups over the past few years [34-40]. Most of the aromatic precursors were synthesized using Grignard reactions while the methine precursor is made through silylation-alcoholysis and the anthracene and ferrocene precursors through lithiation. 2.2.3. Synthesis of organomethylene PMO precursors. (Scheme 4 and 5). Bis(trialkoxysilyl)organic precursors containing methylene groups in the backbone with side-arm functionality have been prepared through lithiation of a bis(triethoxysilyl)methane precursor under nitrogen atmosphere in a freshly distilled anhydrous solvent followed by coupling reactions of the resulting carbanion with various electrophiles (Scheme 4) [72]. [CAUTION: t-BuLi is strongly pyrophoric and should be handled extremely carefully]. This route resulted in a new class of side-arm bridging organosilane precursors. A representative synthetic procedure for the preparation of bromomethylene (BM) and 1,1-bis(triethoxysilyl)-2-(p-bromophenyl)ethane (or pbromobenzyl-methylene) (BBM) PMO precursors are given below. Similar reactions were applied or could be applied to the synthesis of the other precursors shown in Scheme 5. Crude products were used as precursors when distillation resulted in decomposition.
Synthesis of [1,1-bis(triethoxysilyOmethyl] lithium salt (la). A commercially available bis(triethoxysilyl)methane (BTM) (1) was lithiated following a literature procedure [72] with a slight modification. Typically, to 150 mL freshly distilled dry THF was added
bis(triethoxysilyl)methane (BTM, 1) (3.0 g, 8.8 mmol) and the solution was stirred under nitrogen for 5 minutes. Then 5.2 mL of 1.7 M t-BuLi (8.8 mmol BuLi) was added to the above solution dropwise over 10 minutes a t - 78 ~ under a nitrogen atmosphere. The solution was stirred for 1 hr a t - 78 ~ The resulting carbanion lithium salt (la) was subsequently quenched with bromine or 4-bromobenzyl bromide (see below) a t - 78 ~ (Scheme 4 and 5). Scheme 2. Synthetic routes to polysilylated PMO precursors. 1) Grignard Mg / XSi(OR')3 r_
X--R--X
(R'O)3Si~R--Si(OR')3
2) Alcoholysis R'OH
X3Si~R--SiX 3
=
(R'O)3Si--R--Si(OR')3
3) Hydrosilation
~--R---~
(R'O)3Si~
HSi(OR')3,.
, ~R~si(OR')3
H2PtC16 4) Pd-coupling Heck Reaction '----"
X-Ar--X
+ 2
Pd (I) / NEt3
~
\Si(OR,)3
(- HX)
5) Hydroboration
(R'O)3Si-----~__ Ar .v_-
OR)3 BH3.THF
3
or
( ~Si(OR,)3 )
~___ Si(OR')3
l
i(OR')3
H~-----'--~Si(OR,)3
~R'O)3SiJ ~ S i ( O R ' ) 3 6) Lithiation (R'O)3Si~Si(OR')3
t-BuLi / THF .~ -78 C
(R'O)3S i ~ S i ( O R ' ) 3 Li §
R"X
r- (R'O)3Si'~Si(OR')3
R"
7) Silylation of acid halides (acyl halides) C13Si~/SiC13 R~COC1
+ 2 HSiC13
r-
I R
EtOH
(EtO)3Si~/Si(OEt)3
R
Scheme 3. Commercially unavailable precursors used for PMO synthesis (Si stands for
Si(OEt)3). Si Si I Si H
Si~Si
8
9
10
Si Si
Si~ ~-S- S i S
s i ~ S / ~ -Si
11
Si
Si [
Si
.... Si ~/] 12
Fe ~
Si~-.~Si
13
14
Si Si~.v,,'~/'~Si
Si 15
Si H3C~~~ L
H3C
Si H3CO~
--CH3 16
si 20
Si
Si
17
18
F
F
F
F
s. si 21
y "OCH3 Si 19
s si 22
Synthesis of 1,1-bis(triethoxysilyl)bromomethane[(EtO)3SiCHBrSi(OEt)3](BM). To
the carbanion solution (la) was added, a slight excess of bromine (1.5 g, 9.4 mmol) a t - 78 ~ The solution was stirred a t - 78 ~ for 30 min and then at room temperature for 2 hrs. The solvent was removed and the residue was extracted with dry hexane and then filtered. After pumping the solvent off, the residue was vacuum distilled giving bis(triethoxysilyl)bromomethane (3): bp 110-112 ~ / 0.04 mm Hg; IH NMR (300 MHz,
CDC13) 6; 1.21-1.25 (t, 18 H, CH3), 6; 2.18 (s, 1H, CHSi), 6; 3.90-3.96 (q, 12H, CH20); 13C NMR (75.48 MHz, CDC13) 6; 10.13 (CHSi), 6; 18.38 (CH3), 6; 59.62 (CH20); El-MS (m/z) 419 (23%, M+), 375 (25%, [M+- 44]), 163 (100%, [(EtO)3Si+]). Scheme 4. Lithiation of bis(triethoxysilyl)methane and subsequent coupling of lithiated carbanions with organic electrophiles. EEtOXs EtO .... iV
si~Eo Et .....OEt
t-BuLi/THF_ -78 ~
(1)
(la)
(1)
EtO QEt EtO~.\qi &OEt EtO....... ~S_ ......OEt L1
EtEtOksi si~EoEt EtO...... V + .....OEt Li
R'X ~
EtO\ ~Et EtO--~:i ~:i--,OEt EtO....... " ~ ......OEt R'
(2)
(la)
EtO\ EtO~si EtO...... V
~)Et X2 EtO\ ?Et Si~.,OEt .._ EtO,..-. . . . . OEt .....OEt "- EtO......~ly~l""OEt__ Li+ X
R ' M g X EEtONsi Si~.EOEt ._ EtO...... " ~ .....OEt R'
(3)
(la)
R' = D (lb); Br (lc); p-CH2-C6H4Br (ld); p-CH2-C6H4-Si(OMe)3 (le); COOH / COO-Li + (lf); CH2CH2CH2NH2 (lg); Br-camphor (lh); C6F5 (li) (Grignard reaction was also used after lithiation); CH2(CH2)n-i(CF2)mCF3 (lj); CH2NHC6H4NO2 (lk) (See Scheme 5 also).
Synthesis of 1,1-bis(triethoxysilyl)-2-(p-bromophenyl)ethane (p-bromobenzylmethylene precursor) [(EtO)3SiCH(CH2-p-C6H4BOSi(OEt)3] (BBM). To la was added a THF (10mL) solution ofp-bromobenzylbromide (2.2 g, 8.8 mmol) a t - 78 ~ After similar work-up as above, BBM was obtained: bp 144-148 ~ / 0.04 mm Hg; 1H NMR (300 MHz, CDC13) 6 0.55-0.58 (t, 1 H, CHSi), 8 1.18-1.23 (t,18H, CH3), 8 2.89-2.92 (d, 2H, CHzPh), fi 3.78-3.82 (q, 12H, CH20), ~ 7.17-7.20 (d, 2H, ArH), 6; 7.36-7.39 (d, 2H, ArH); ~3C NMR (75.48 MHz, CDCI3) fi 10.80 (CHSi), 6; 18.46 (CH3), 6;29.47 (CHEPh), 8 58.66 (CH20), 6130.84, 131.10 (CH aromatic); EI-MS (m/z) 508 (5%, M+), 464 (100%, [M +- 44]).
Scheme 5. Synthesis of PMO precursors with organomethylene groups in the framework. lh
(R'O)3.Si~Si(OR')3
(R'O)3Si'~Si(OR')3
~'H2
3c'a%dpLboTm~
]
(R'O)3Si~ISi(OR')3
lo
O~---O-Li§
Si(OMe)3 CO2 C1CH2
(R'O)3Si~-~Si(OR')3 [
/Si(OMe)3
(~U2Br !(R' !................................... O)3Si~Si(OR' [ )3 ] 1CH NH"(R'O)3Si'~Si(OR')3 i "+ [ C( 2)3 2 CH2(CH2)2NH2
~~1
[.................Li..........~p...j
CF3(CF2)m(CH2)nC1 /
D20
/ NHCH2CI / ~
Br2~
(R,O)3Si~.~Si(OR,)3
~I CH2(CH2)n-1 (CF2)mCF3 (R'O)3Si Si(OR')3 lj
(R'O)3Si~-Si(OR')3 NO2 ~FsMgBr CH2 I IH (R,O)3Si~...Si(OR,)3 (R'O)3Si'~Si(OR')3 D F~F lk lb li F F NO2 F 2.3. Self-assembly of BM and other PMOs under acidic conditions For a typical synthesis under acidic conditions, a solution of cetyltrimethylammonium bromide (0.34 g, 0.93 mmol), HC1 (7.18 g, 36 wt%, 70.8 mmol) and water (13.4 g, 0.74 mol) was prepared at room temperature (Scheme 6). To this solution was added 3.85 mmol (or 7.70 mmol Si) of the required precursor and the mixture was stirred for 30 mins. After aging at 80 ~ for 4 days, the product was isolated by filtration, washed with copious amounts of water, and dried under ambient conditions. (For bromomethine a light brownish powder was obtained with a typical yield of 0.56 g).
2.4. Self-assembly of B B M and other P M O s under basic conditions
A solution of cetyltrimethylammonium bromide (0.67g, 1.84 mmol), ammonium hydroxide (14.18 g, 35 wt%, 0.14 mol) and water (26.73 g, 1.48 mol) was prepared at room temperature (Scheme 6). To this solution 2.94 mmol (or 5.88 mmol Si) of precursor was added (for 50% BBM PMO, 2.94 mmol BBM and 1.47 mmol of TEOS) and the solution was stirred for 30 minutes during which time a precipitate formed. After aging at 80 ~ for 4 days, the product was filtered, washed with copious amounts of water, and dried under ambient conditions resulting in a fine powder (typical yield of 0.49 g of white powder was obtained for bromobenzyl-methylene PMO). Scheme 6. Synthesis and solvent-extraction of BM and BBM PMOs
EE~~si si~EoEt EtO " x ~ .....OEt
CTABr/ +/H20 . . . . . .
oS
Lo
O""Si~ Si''''O
Br
Br
lc
lc'
EtO\ ~Et EtO.---Si qi-,-OEt EtO"" x ' ~ ......OEt +
02,
.OEt EtO~S,i"OEt
CTABr/ OH-/H20
HCI / MeOH ..... =
BM PMO
......o
H2
HC1/ MeOH = BBM PMO
OEt
Br ld
Br ld'
2.5. Surfactant-extraction of P M O s
The surfactant was removed from the samples using solvent-extraction in an HC1/methanol solution. Typically ca. 0.3 g of as-synthesized powder was stirred for 6 hrs at 55 ~ in a solution of 4 g of conc. (36 wt %) HC1 and 170 g methanol. The product was then isolated by filtration, washed with methanol, and dried in air. A typical weight loss of ca. 30 % was obtained for each sample after a single solvent extraction. The surfactant removal was confirmed by solid-state 13C CP MAS NMR. 2.6. Instrumentation and characterization techniques
The as-synthesized and surfactant extracted materials were characterized using powder X-ray diffraction (PXRD), transmission electron microscopy (TEM), 13C, 29Si CP MAS (29Si MAS as required) and 79Br MAS NMR, N2 adsorption, thermogravimetric analysis (TGA), and elemental analysis (EA).
10 Powder X-ray diffraction (PXRD) patterns were measured with a Siemens D5000 diffractometer using Ni-filtered Cu-K~ radiation with )~ = 1.54178 A. The high temperature in-situ measurements were done as reported in Ref. [8]. TEM images were recorded on a Philips 430 microscope operating at an accelerating voltage of 100 kV. Nitrogen adsorption measurements were carried out at 77 K on a Micromeritics ASAP 2010 volumetric adsorption analyzer. Before the measurements, the samples were degassed under vacuum at 100 or 140~ Weight change curves were obtained under nitrogen or air atmosphere on a TA Instruments TGA 2950 thermogravimetric analyzer (TGA) using a high-resolution mode with a maximum heating rate of 5 ~ min -1. Solution phase nuclear magnetic resonance spectra were taken with a Varian VXR 300 spectrometer. Solid-state NMR spectra 13C CP-MAS (100.6 MHz), 29Si CP-MAS (79.5 MHz) and 79Br MAS NMR (100.3 MHz) were obtained with a Bruker DSX400 spectrometer. Experimental conditions: 13C CP-MAS NMR (6.5 kHz spin rate; 2.5 ms contact time; 3 s recycle delay; 10,000-20,000 scans); 13C NQS (non-quaternary suppression) CP-MAS NMR experiment, 6.5 KHz spin rate, 3 s recycle delay, 50 ~ts dephasing delay, 5,000-10,000 scans; 29Si MAS NMR (6.5 KHz spin rate; 100 s recycle delay; 800-1000 scans). 29Si CP MAS NMR experiments: 6.5 kHz spin rate, 3 s recycle delay, 10 ms contact time, zr/2 pulse width of 6.0-7.5 ~ts, 200-5,000 scans. 79Br MAS NMR (6.5 KHz spin rate; 0.1 s recycle delay; 50,000-100,000 scans). 3. R E S U L T S A N D D I S C U S S I O N 3.1. Precursor synthesis Since the reports on the first PMOs [1,2,13,18]; we have been actively investigating the possibility of incorporating other organic functional groups into the framework of PMOs. Some of the challenges are briefly described here. As most PMO precursors were not commercially available, their synthesis under inert atmosphere was routinely required. Most of the poly(trialkoxysilyl)organic precursors discussed in this article were prepared through lithiations and Grignard reactions while some are commercially available. We found that the synthesis through lithiation usually resulted in higher yields than the analogous Grignard reactions. The required precursors were usually isolated and purified by distillation under vacuum to avoid possible decomposition due to their rather high boiling points under standard conditions. The reaction of lithiated carbanion solution (la) with electrophiles was found to be quite favorable and resulted in good yields when the reaction was carded out rigorously under an inert atmosphere. 3.2. Synthesis of PMOs 3.2.1. Linear unsaturated and saturated organic bridge-bonded PMOs So far, the literature reported PMOs have rigid and/or short organic groups. These were found to result in rather well ordered mesoporous structures. For instance, we reported the synthesis of the shortest organic bridgebonded PMOs (1) with 2-D hexagonal mesostructures (Figure 1) containing methylene bridges that are isoelectronic with oxygen atoms in MCM-41 materials [3]. We also recently expanded the synthetic route to include cubic [10] and biphasic (hexagonal and cubic together in the same material) methylene PMOs. Figure 1 shows the powder X-ray diffraction (PXRD) pattems and TEM images for various methylene PMO structures. The thermal
11 transformation of bridging methylene into terminal methyl groups in these PMO materials is particularly interesting and provides a novel route to new organic functionalized mesoporous materials with high loadings of functional groups. Similarly, we prepared an ordered mesoporous methine PMO (8) with the methine groups bridging three silicate units in a mesoporous structure (Scheme 3). The precursor for this PMO (8) was prepared by silylating chloroform in the right stoichiometry followed by alcoholysis as reported by Corriu et al. [72]. (A) Methylene PMO (hexagonal and cubic)
(C) Hexagonal methylene PMO
(B) Methylene PMO (biphasic)
(D) Cubic methylene PMO
Figure 1. PXRD patterns of hexagonal, cubic and biphasic methylene PMOs (A, B) and TEM images hexagonal and cubic methylene PMOs (C, D) PMOs with two carbon bridging organic groups were among the first to be reported. They included ethane (2), ethylene (3) and acetylene (12) PMOs [1,2,13-18]. 2D hexagonal, 3-D hexagonal and cubic structures were reported for 2 [ 13-16], both 2-D
12 hexagonal and disordered structures were reported for 3 [1,18], while most of the Si-C bonds were found to cleave for 12 [2]. The ability to vary both the composition and the structures of the materials will offer numerous opportunities for applications. Ethane PMOs were also reported to adopt various curved morphologies [25,26], which will likely be useful in separation applications. Furthermore, accessibility and reactivity of ethylene group in an ethylene PMO were demonstrated with bromination [1,18] and hydroboration [ 12] reactions giving more opportunities for further functionalization. For instance, the 13C NMR and 29Si CP MAS NMR spectra for ethylene PMO before and after hydroboration (Figure 2) indicate that some of the ethylene carbons are available for reaction with the retention of the periodic structure (see PXRD patterns in Figure 2A).
(B) t3c CP MAS NMR spectra
(A) PXRD patterns lOOOl~,
- Jll, ~, ~
"
Solvent-extracted
~
//
Hydroborated (Spin i~'ate= 8"()KHz
l] 1
tlydmborated (SpinRate = 6.5 KHz)
Hydroborated
20(0) (C) '~Si CP MAS NMR spectrum
/
II~
e
S~
borated " " * " ' ~ ' ( " ' ' " ' 1
150 I
";"
"
I
. . . . .
|
. . . .
....
100
~'1
. . . .
50
I'"
0
I
o -so -too .1so Chemical shift (ppm)
Chemical shift (ppm)
Figure 2. A) PXRD pattems of ethylene PMO before and after hydroboration; B) 13CCP MAS and (C) 29Si (CP) MAS NMR spectra of ethylene PMO before and after hydroboration. PMOs containing a bridging group with one or two carbon atoms as well as other rather short and rigid organic groups were observed to self-assemble quite readily and form well-ordered structures. Further investigations in our group revealed that poly(trialkoxysilyl)organic precursors having bridging organic groups with four or more carbon chains did not self-assemble and gave only amorphous gels and disordered materials. For instance, 2-butylene (16), hexylene (5), 1,4-diethylbenzene (6), and N,N'dipropylethylenediammine (7) bridge bonded materials when templated with surfactants were all found to be amorphous with no low angle Bragg reflections. However, three
13 carbon chain precursor materials with bridging organic groups like 1,1dimethylvinylidene (4) were found to give partially ordered PMO materials. These observations indicate that the more flexible and non-polar bridging organic groups partially or fully prevent the development of mesoscopic order during surfactant templated self-assembly. Attempted synthesis of 2-butylene with large head group surfactants (cetyltriethylammonium bromide) [73] also failed to produce well-ordered PMO materials.
3.2.2. Aromatic and organometallic bridge bonded PMOs various kinds of aromatic and organometallic PMOs [2,9] with ordered mesoporous structures and some of these with a certain degree of additional spatial ordering of the aromatic groups in the pore walls due to re-re stacking, (as indicated by Xray diffraction data [9]) have been synthesized and reported. For instance, we have prepared 1,4-phenylene (9) [2], 1,3,5-phenylene (14) 2,5-thiophene (10) [2], 2,2'bithiophene (11) [2], 1,4-xylyl (17) [9], 1,4-(2,5-dimethylphenylene) (18) [9], 1,1'ferrocene (13) [2], and 1,4-(2,5-dimethoxyphenylene) (19) PMOs [9]. In addition, ptoluyl (20), 1,4-perfluoroaryl (21) and 2,5-pyridine (22) PMOs have also been prepared but their structures were not well defined and their stability was poor. The synthesis conditions for most of the aromatic PMOs should be chosen carefully in order to avoid or minimize cleavage of Si-C bonds. For example, significant cleavage of Si-C bonds was observed in thiophene, bithiophene and ferrocene PMOs. Aromatic groups within these PMOs are potentially useful as good supports and carriers for metal or organometallic guest molecules, which may ultimately be useful as catalysts (for example pyridine is a good ligand for anchoring metals). Some of the organics are also known to have high affinities for many other organic molecules, a property that could make this class of PMOs useful for separation and environmental remediation applications. Moreover, conjugated aromatic and organometallic containing PMOs based on anthracene (15) and ferrocene (13) could find applications as sensors as they contain optically active and electroactive moieties. 3.2.3. Organomethylene bridge bonded PMOs Recently, we have prepared a new class of PMOs with star-like organic bridging groups based on a methylene backbone. It is known that methylenesilica PMOs were amongst materials with well ordered mesoporous structures and interesting properties and we have chosen these groups as platforms to attach various functional groups (Schemes 4 and 5). These reactions were carried out by taking advantage of the lithiation reactions that bis(trialkoxysilyl)methane undergo resulting in the corresponding carbanion (la) allowing one to replace one of the protons by other active organic molecules. This opened an avenue to a diverse group of functionalized PMOs including heteroatom containing organic groups. Some examples of PMOs whose synthesis was attempted by this route include bromomethylene (lc), p-bromobenzyl-methylene (ld), p-benzylmethylene (le), carboxylic acid-methylene (If), (+)-bromocamphor-methylene (lh), and perfluoaryl-methylene (li) PMOs. The synthesis of PMOs with these groups would afford some of the first mesoporous materials with highly reactive bridge bonded organic groups in the framework and protruding into the void spaces. Each of these materials is anticipated to have their own special properties and particular applications. For example,
14 the (+)-bromocamphor is a chiral group and could be useful for chiral reactions, catalysis and separations. The benzyl-methylene PMO is a new type of aromatic PMO with three surrounding silicate units unlike most of the previously discussed aromatic PMOs. The perfluoraryl (li) and perfluoroalkyl (lj) functional groups will make the PMO materials more hydrophobic and "Teflon-like" and could lead to a new class of low dielectric constant materials. Our preliminary investigation on perfluoraryl-methylene PMOs (li) was promising but more work is needed to determine their stability and properties. The other reactions in Scheme 5 that will not be discussed in detail here but are worth mentioning involve those carrying basic (lg), acidic (If) and optically non-linear (lk) functional groups on the methylene bridging group. Each of these PMOs would be interesting as an advanced material for various applications. (A) Methine PMO (solvent-extracted)
(B) p-Benzyl-methylene PMO (solvent-extracted)
~
IlL
9 .... 2
~.~t,~ ~ 4
.
. 6
.
.
.
t
. 8
.
l(i
0 5
1o
20 (degrees)
10
15
20
2A
.~0
2e (degrees)
(C) Other PMOs (solvent-extracted) 3OO0
ga, 2~m .,.., ~ l~D.~v~. I ,
/
Bromocamphor-methylene PMO
[
-Dime, y vm leae. , o
0 .....
-.~-~.~..-~,o.~.. ,. . . . . 5
,
..
.
!0
..
, 15
-~ ............. 20
20 (degrees)
Figure 3. PXRD pattems of various PMOs with organomethylene groups in their frameworks. The synthesis of the aforementioned PMOs was performed and PXRD patterns of most of the resulting materials after template extraction using acid/methanol washing showed at least one low angle Bragg peak indicating the presence of an ordered mesoporous structure (Figure 3). For some of these materials, the porous structure was additionally studied using nitrogen adsorption. The sample synthesized using the
15 bromocamphor-methylene precursor was clearly mesoporous (see adsorption isotherm in Figure 4A) and exhibited primary mesopores of diameter about 3.6 nm, a very large BET specific surface area (1310 m 2 g-l) and a significant total pore volume (0.99 cm 3 g-l). However, as will be discussed below in more detail, this PMO was found to contain only a small amount of bromocamphor-methylene bridging groups, whereas its predominant bridging group was methylene. The presence of very limited amount of bromocamphor groups can be inferred from a small magnitude of TGA weight loss (Figure 4B). Therefore, this sample can be referred to as methylene/bromocamphor-methylene PMO. The attempted synthesis of benzyl-methylene PMO (le) in which a bridging organic group connected to three silicon atoms resulted in a mostly microporous material with the BET specific surface area of 670 m 2 g-i and a total pore volume of 0.41 cm 3 g-1. The surfactant-extracted sample exhibited a small weight loss related to the decomposition of the residual surfactant at about 200~ followed by a very large weight loss that can be primarily related to the decomposition and thermodesorption of large organic groups in the PMO structure. The synthesis of a 1,1-dimethylvinylidene PMO (4) was also attempted and the resultant solvent-extracted sample was mesoporous (pore diameter of about 2.6 nm) and exhibited an appreciable adsorption capacity despite the fact that a certain amount of surfactant was not removed, as seen from TGA. As will be shown below, an appreciable degree of cleavage of Si-C bonds took place during the synthesis of this material, and therefore it is expected to have a significant amount of pendent rather than framework organic groups (the retention of organic groups can be inferred from TGA data; additional evidence for preservation of Si-C linkages is presented below) The presence of bridging organic groups in these PMOs, were investigated using solid-state NMR spectroscopy. The 13C CP MAS NMR (Figure 5), for instance, indicates the presence of small percentages of bromocamphor-methylene and a large quantity of methylene not containing camphor groups probably because the crude product was used as a precursor in this case. Further, large percentages of functional groups were observed in methine (8) and 1,1-dimethylvinylidene (4) PMOs. The methine PMOs also showed similar thermal~ stability to those of methylene PMOs and the surfactant template in these materials was easily removed with calcination in air at 350 ~ Template removal in acid/methanol solution for 1,1-dimethylvinylidene PMO causes hydrochlorination of the vinyl carbons unless carried out under very mild acidic solution. The 29Si CP MAS NMR spectrum (Figure 6) of the sample synthesized using the bromocamphor-methylene precursor showed essentially only T sites, thus revealing no Si-C bond cleavage. However, most of the other materials exhibited a cleavage of Si-C bonds, which was significant for instance for 1,1-dimethylvinylidene and methine PMO, in which case as much as about 50% of these bonds could have been cleaved. In what follows, we will focus on similarly prepared bromo- and p-bromobenzylfunctionalized methylene PMOs where bromo and organobromo sites are attached to bridging methylene groups. Organohalides are well known to undergo various reactions such as lithiation, Grignard and metal-catalyzed coupling and the organohalide functional groups in PMOs are likely to undergo similar reactions allowing further surface, chemical and physical modifications and making catalytic activity, ion-exchange and easily surface-modifiable materials possible. This property makes these materials the first examples of highly reactive PMOs due to the ease of substitution of bromides by other interesting functional groups and ligands.
16 100 -'-' 700 f melhylenei ' i A) " '~0 Lbr~176176 600 / m e t h y l e n e ~ l , 1-dimethyl- " r.~ ~ 500
90 80
..~methyiene/bromocamphorlene
~
._~ 1,1-dimethyl"x,.X.... . .vinylidene ................
(B)
400 "~
300
PMO \ \
60
200 t~ 100 <
7o
F
\\ benzyl
benzyl
\
50 _
0.0
i
i
I
i
0.2
0.4
0.6
0.8
Relative Pressure
1.0
I
I
I
I
200
400
600
800
1000
Temperature (~
Figure 4. (A) Nitrogen adsorption isotherms and (B) weight change curves under air atmosphere for methylene/bromocamphor-methylene, 1,1-dimethylvinylidene and benzyl PMOs. The PXRD pattems of as-synthesized and surfactant extracted bromomethylene (BM) and p-bromobenzyl-methylene (BBM) PMOs (Figure 7) reveal a low angle Bragg peak consistent with the presence of an ordered mesostructure. The former was synthesized under acidic conditions and the latter with 50% TEOS under basic conditions. Attempted synthesis of BM PMO under basic conditions failed to give a high yield of ordered material possibly because of the formation of soluble salts that remained in the supematant. The PXRD pattern of BBM PMO containing 50% TEOS, made under basic conditions showed an intense (100) reflection as well as visible (110) and (200) Bragg peaks indicating the presence of long-range mesoscopic order (Figure 7B). The cocondensation of the BBM precursor with TEOS might have accounted for better selforganization resulting in a more well ordered material, but there might also be some chances that phase separation took place forming an ordered phase that was not particularly rich in the bridged organosilicate groups. The structure of the material synthesized from 100% BBM precursor under the same conditions was a somewhat disordered material under the same conditions. The positions of the main XRD reflection (dl00) for surfactant-extracted BM and BBM/TEOS PMO were ca. 34.3 and 42.7A, respectively. The structure of surfactant-extracted BBM PMO when pyrolyzed in a nitrogen atmosphere and monitored in situ by PXRD revealed that the ordered structure was maintained up to 900 ~ (Figure 7C). A broadening of the main PXRD reflection, and unit cell dimension (ao = 2d100/~/3) from 49.3 to 35.8 A were observed during calcination of the material from RT to 1000 ~ The retention of PXRD intensity up to at
17 least 700~ may be related to the loss of the organic groups, thereby increasing the electron contrast between the framework and the void space, while the slow decrease in d-spacing from 200 to 1000 ~ was consistent with the condensation of residual silanol SiOH groups, and loss of the organic framework groups. The TEM images of these materials also showed some ordered hexagonal structure with some fraction of amorphous regions. The 13C, 298i CP MAS (29Si MAS as needed) and 79Br MAS NMR spectra of BM and BBM PMOs are shown in Figures 8, 9, and 10, respectively and the results are summarized in Table 1. Table 1. Chemical shift assignments for BM and BBM PMO materials Sample 13C CP MAS (ppm) 29Si MAS (ppm) 79Br MAS (ppm) 10 -72 ppm- T3 -300 ppm (broad) BM-PMO (-2 and 26) -67 ppm- T2 CHBr -57 ppm- T1 -365 ppm (sharp) B r 14 - 100 ppm - Q4 -300 ppm (broad) 29 -101 ppm - Q3 CHBr 120 -91 ppm - Q2 -365 ppm (sharp) B r BBM-PMO 131 -73 ppm- T3 142 -67 ppm - T2 -57 ppm- T1 The 13C CP MAS NMR spectra of BM PMO (Figure 8) prepared under acid conditions showed a peak at 10 ppm corresponding to (O3Si)2CHBr carbons, a Chemical shift consistent with solution NMR results (see Experimental). An additional peak at 26 ppm observed in the spectrum was attributed to (O3Si)2CHC1 and resulted from nucleophilic substitution of Br by C1 during self-assembly of BM under acid (HC1) conditions and to some extent during solvent extraction in an HC1/MeOH solution. Due to the many similarities in reactivity between the two halogen atoms, Br and C1, both bromomethylene and chloromethylene groups in the PMO could show similarities under most instances. However, slight differences in reactivity due to steric and electronic differences cannot be ruled out and can be taken advantage of for making multifunctional materials where one reacts selectively over the other under certain conditions. The 13C CP MAS NMR spectra (Fig 8B) also showed peaks consistent with p-bromobenzylmethylene groups. Peaks at 14 and 29 ppm were assigned to (O3Si)2CHCH2-p-C6H4Br and (O3Si)2CHCH2-p-C6H4Br carbons while peaks at 120, 131, and 142 ppm were attributed to aromatic carbons. A minor peak or shoulder at 1 ppm was also observed in both materials that corresponds to methylene carbons that were formed probably due to radical substitution of Br by H in BM PMO and cleavage of the p-bromobenzylmethylene group in BBM PMO. 29Si MAS and CP MAS NMR spectra (Figure 9) indicated that the Si-C bonds of the materials remained intact during the synthesis and surfactant extractions. The 29Si (CP) MAS NMR spectra also showed that BM PMO has only T sites while BBM PMO has a T:Q ratio of ca. 1:1 consistent with the ratio of starting alkoxy/poly(trialkoxy)organosilanes.
18 (A) Bromocamphor-methylene PMO
(B) 1,1-Dimethylvinylidene PMO
Solvent-extracted,
Solvent-extracted, "C CP MAS
/~ ...... i 150
......
,
. . . .
~ . . . .
100
50
, ' '
ppm
Solvent-extracted,
.
.
.
.
I
.
.
.
.
!
150
~
~'-
leO
"
I
.
.
.
.
i
50
'''J
.......
' '
""
!
. . . .
150
O
Chemical shift (ppm)
t
" ' '
100
"
I
50
. . . .
!
"
'
0
Chemical shift (ppm)
(C) Methine PMO
Calcined, 350 "C, ~3CCP MAS i .....
....
100
'"
"
"
"
I
. . . .
~ .... 50
!
. . . .
~'"
ppm
l
'
As-synthesized, I~CNQS CP MAS
~
leo
As-synthesized, ~3CCP MAS . . . .
1
. . . .
1O0
I
50
. . . .
!
"
"
0
Chemical shift (ppm)
Figure 5. 13C CP MAS NMR spectra of various PMOs with organomethylene and methine groups in their frameworks.
19 (A) Bromocamphor methylene PMO (solvent-extracted) (B) 1,l-Dimethyvinyledene PMO (solvent-extracted)
[
~.~
9 .v~
.~,-
,
I
"
~
' '
'
I
"
'
"
0
"
0 -5tj -100 Chemical shift (ppm)
-50 -100 Chemical shift (ppm)
(C) Methine PMO
9 reed " 350 "C
I'"'"
'
"
'
i
. . . .
-50
I
. . . .
-100 ppm
ctant-extracted
i--'-
O
'
'
'
I
. . . .
I
. . . .
-50 -10O Chemical shift (ppm)
Figure 6. 29Si CP MAS NMR spectra of various PMOs with organomethylene and methine groups in their frameworks.
Investigations using 79Br MAS NMR spectroscopy for the as-synthesized materials revealed the presence of bromides corresponding to both organobromine groups as well as bromide counterions for the surfactant head groups (Figure 10) (as expected for the BM sample because of the self-assembly under acidic conditions, where surfactant is known to be incorporated with counterions [45]). Interestingly, the peak at - 300 ppm corresponding to bromides of the organobromine groups appeared to have a larger line width than the peaks a t - 365 a n d - 398 ppm corresponding to bromide ions from the CTABr surfactant. This is most likely due to the fact that the organobromine groups are covalently attached and are therefore more rigid than the bromide counter-ions. The
20 presence of more than one sharp peak corresponding to Br- ions (surfactant counterions) is consistent with the presence of various kinds of bromides in different environments in the materials. Most of these sharp peaks corresponding to free bromide ions of the surfactant disappear or their intensity decreased significantlyupon solvent-extraction, as expected. (A) Bromomethylene PMOs
(B) p-Bromobenzyl-methylene PMOs
jt~l
4oo~
d,,,
3()IH~
~"
=.
I ~ ~,,~., S o l v e n t - e x t r a c t e d
'~176 t
)
"-"
)' ~.~
As-synthesized
j
:'~
'10~
k,.
...1............ 10
Solvent-extracted
20
As-synthesized
0 ..................................................................... r ........................." ~ ' ~ 10
30
20 C)
.......................................i
20
20 (")
(C) p-Bromobenzyl-methylene PMOs dloo
3000~
....___~ 20000
900~ 800 *c
700~ j
6oo*c 500"C 400"C 350"C 300 "C 200 ~'C 25 "C
-~,~
10000
o
............
;, .............. ~, ....
~
"
io
...... i2
....
'1'4'
20( ~) Figure 7. Powder X-ray diffraction pattems of (A) bromomethylene PMOs; ( B ) p bromobenzyl-methylene PMOs (BBM PMO); (C) surfactant extracted BBP PMOs monitored during high temperature in-situ pyrolysis under nitrogen from RT to 1000 ~ Elemental analysis (EA) of the materials indicated that the wt% of Br was 20.05 and 25.25 for the as-synthesized and surfactant extracted BM PMO, respectively and 24.23 for surfactant extracted BBM PMO samples. Moreover, 5.70 and 3.01 wt % C1 was obtained for as-synthesized and surfactant-extracted BM-PMO material proving the substitution of some of the bromides by chlorides, which is consistent with the 13C CP
21 MAS NMR spectra. The EA results indicated that the Br:C1 ratio for solvent-extracted material is c a . 4:1. Combining the NMR and elemental analysis results, we estimated (Ol.5SiCHBrSiOi.5)o.73(Oi.5SiCHC1SiOl.s)o.18(Ol.sSiCHzSiOi.5)o.09 to be the composition of the surfactant extracted material.
(A)
Bromomethylene PMO
(B) p-Bromobenzyl-methylene PMO
Solvent-extracted, t3
,,
"
"
"
"
'
R
Solven~ 2(10
150 ,
l~t0 5'0 ('~ Solvent-extracted, ~', ? ~
6o
l[o
lbo
sb i
6
~] As-synthesized, As-synthesized ~ 150
50
r------
0 Chemical shift (ppm)
..... i . . . . . . . . .
200
:!
150
!
100
.............l ..............
50 Chemical shift (ppm)
i ....
0
Figure 8. 13C CP and NQS CP MAS NMR spectra of (A) bromomethylene PMOs, assynthesized (a) and surfactant extracted (b); (B) bromobenzyl-methylene PMOs, assynthesized (a) and surfactant extracted (b, c). Both BM and BBM PMO samples exhibited rather moderate specific surface areas of 500 and 650 m 2 g-i, respectively, and total pore volumes (0.23 and 0.39 cm 3 g-i, respectively). BM PMO was microporous with average pore diameter around 1.6 nm, whereas BBM PMO was mesoporous with a very broad pore size distribution centered at around 3 nm. Adsorption properties of a porous silica obtained from the BBM PMO sample via calcination deviate from those of MCM-41 silicas. This may be due either to a prominent wall corrugation for the BBM PMO sample (or introduced during calcination) or to the presence of some disordered domains in the material, as suggested by TEM images and additionally supported by the fact that the isotherm for BBM is somewhat atypical for a 2-D hexagonal material. TGA for BM PMO corroborates the elemental analysis data, suggesting that bridging groups account for an appreciable fraction of the mass of the sample. Moreover, the comparison of TGA data for as-synthesized and surfactant-extracted BM PMO reveal an appreciable weight loss attributable to the surfactant decomposition, thus strongly suggesting that this is a supramolecularlytemplated material despite its microporous nature and unprecedented content of heteroatoms in the structure. BBM PMO sample exhibits a moderate weight loss in the temperature range for decomposition of the bridging groups. Apparently, its content of
22 bromobenzyl groups is significantly lower than that expected from the composition of the synthesis gel. (A) Bromomethylene PMO
(B) p-Bromobenzyl-methylene PMO (Solvent-extracted)
xtracted (~Si MAS)
-so
-ioo -1 o MAS NMR
Solvent-extracted ("~SiCP MAS)
6
-so
:ioo ,1so ~'Si CP MAS NMR
~-s~esized
("Si CP MAS)
6 I)
-50
-i00
.;o
.~bo
-1~o
-1.50 Chemical shift (ppm)
Chemical shift (ppm)
Figure 9. 29Si (CP) MAS NMR spectra of (A) bromomethylene and (B)p-bromobenzylmethylene PMOs. (A) Bromomethylene PMOs
(B) p-Bromobenzyl-methylene PMO
,
t-extracted
; .... -Ioo
~
I,
nt-extracted
2g
- '40O
a,.
nthesized
ynthesized .
!
Chemical shift (ppm)
i}
20o
.
.
.
.
44H~
~
Chemical shift (ppm)
Figure 10. 79Br MAS NMR spectra NMR spectra of (A) bromomethylene and (B)pbromobenzyl-methylene PMOs.
23 Attempted in-situ reactions of BM PMO with ammines, Na28204, NaHS.xH20 and other reagents indicated that the CHBr groups are chemically accessible. However, the Si-C bonds were found to cleave causing the collapse of the structures under some of these reactions. Further investigations will be required to find the optimum conditions to leave the Si-C bonds and the structure intact during some of these in-situ reactions. 100 "7
~0 250
r./3
(A) 90
p-bromobenzylmethylene PMO
200
~.
150 9 r~
"~ <
100
~
50
~
.,.~ O
bromomethylene PMO
~:
,
(B)
i
,
,
", p-bromobenzyl\,m,ethylene PMO
80 70
omethylene PMO
6o "'..s~nt-extracted 50
as-synthesized'" .................... 0 0.0
. 0.2
.
. 0.4
. 0.6
Relative Pressure
40 0.8
1.0
0
i
i
i
i
200
400
600
800
1000
Temperature (~
Figure 11. (A) Nitrogen adsorption isotherms and (B) weight change curves under air atmosphere (except for the one for as-synthesized material, which was recorded under nitrogen) for BM and BBM PMOs. Successful in-situ reactions in ordered PMOs and bifunctional PMOs (BPMOs) have been reported as new routes to funtionalized PMOs and BPMOs which otherwise might be hard to make by direct synthesis [1,8,12,18]. With these approaches, dibromo, borylated, epoxide, diol and alcohol functionalized materials have been synthesized. The borylated and epoxide functionalized PMOs particularly are important materials as they undergo further transformations to yield several other functional groups and under mild conditions. For instance, they are proven to undergo chemical transformations into alcohol functionalized mesoporous materials [8]. Preliminary experiments [12] also indicated that the amine-functionalized mono- and bifunctional PMO materials can form by treating a borylated bifunctional PMO material with hydroxylamine-o-sulphonic acid. Amine functionalized mesoporous materials can be useful materials as base-catalyst, acid scavengers and sensors. 4. CONCLUSIONS In this paper we have reviewed recent work, mainly from our laboratory, on a new class of hybrid organic-inorganic mesoporous materials called periodic mesoporous organosilica (PMOs) containing bridge bonded organic groups integrated into the frameworks. These materials show a number of unique properties including high loading of bridging organic groups, large free void space and a uniform distribution of functional
24 groups in the framework. Some of the functional groups are accessible to further chemical modification. The presence of bridging organic groups in PMO frameworks is expected to result in interesting physical and mechanical properties as well as useful chemical functionality that make PMOs potentially useful for diverse applications including catalysis, sensing, separations and nanoelectronics. 5. ACKNOWLEDGMENTS GAO is a Canada Research Chair in Materials Chemistry. He acknowledges the financial support of the National Science and Engineering Council of Canada (NSERC) for financial support of this project. MJ acknowledges the financial support from NSF Grant CHE-0093707. The authors would also like to thank Prof. Mark. J. MacLachlan, Stephen Knauer, Chiaki Yoshina-Ishii, Galina Temtsin, Prof. Shmuel Bittner, Dr. Masakatsu Kiroki, Dr. Srebri Petrov, Dr. Neil Coombs, Wesley Whitnall, and Rebecca Voss for their contributions and helpful discussions. REFERENCES 1. T. Asefa, M. J. MacLachlan, N. Coombs and G. A. Ozin, Nature, 402 (1999) 867. 2. C. Yoshina-Ishii, T. Asefa, N. Coombs, M. J. MacLachlan and G. A. Ozin, Chem. Commun., (1999) 2539. 3. T. Asefa, M. J. MacLachlan, H. Grondey, N. Coombs and G. A. Ozin, Angew. Chem. Int. Ed., 39 (2000) 1808. 4. M.J. MacLachlan, T. Asefa and G. A. Ozin, Chem. Eur. J., 6 (2000) 2507. 5. T. Asefa, C. Yoshina-Ishii, M. J. MacLachlan and G. A. Ozin, J. Mater. Chem., 10 (2000) 1751. 6. T. Asefa, N. Coombs, t3. Dag, H. Grondey, M. J. MacLachlan, G. A. Ozin and C. Yoshina-Ishii, Mater. Res. Soc. Symp. Proc., 628 (2000) CC3.9. 7. O. Dag, C. Yoshina-Ishii, T. Asefa, M. J. MacLachlan, H. Grondey and G. A. Ozin, Adv. Funct. Mater., 3 (2001) 213. 8. T. Asefa, M. Kruk, M. J. MacLachlan, N. Coombs, H. Grondey, M. Jaroniec and G. A. Ozin, J. Am. Chem. Soc., 123 (2001) 8520. 9. G. Temtsin, T. Asefa, S. Bittner and G. A. Ozin, J. Mater. Chem., 11 (2001) 3202. 10. T. Asefa, M. Kruk, N. Coombs, S. Petrov, M. Jaroniec and G. A. Ozin, unpublished results. 11.13. Dag and G. A. Ozin, Adv. Mater., 13 (2001) 1182. 12. T. Asefa, M. Kruk, M. Jaroniec and G. A. Ozin, unpublished results. 13. S. Inagaki, S. Guan, Y. Fukushima, T. Ohsuna and O. Terasaki, J. Am. Chem. Soc., 121 (1999) 9611. 14. S. Guan, S. Inagaki, T. Ohsuna and O. Terasaki, J. Am. Chem. Sot., 122 (2000) 5660. 15. S. Guan, S. Inagaki, T. Ohsuna and O. Terasaki, Microporous Mesoporous Mater., 44 (2001) 165. 16. S. Inagaki, S. Guan, Y. Fukushima, T. Ohsuna and O. Terasaki, Stud. Surf. Sci. Catal., 129 (2000) 155. 17. A. Fukuoka, Y. Sakamoto, S. Guan, S. Inagaki, N. Sugimoto, Y. Fukushima, K. Hirahara, S. Ijima and M. Ichikawa, J. Am. Chem. Soc., 123 (2001) 3373.
25 18. B. J. Melde, B. T. Holland, C. F. Blanford and A. Stein, Chem. Mater., 11 (1999) 3302. 19. Y. Lu, H. Fan, N. Doke, D. A. Loy, R. A. Assink, D. A. LaVan, and C. J. Brinker, J. Am. Chem. Soc., 122 (2000) 5258. 20. H. Fan, S. Reed, T. Baer, R. Schunk, G. P. Lopez and C. J. Brinker, Microporous Mesoporous Mater., 44 (2001) 625. 21. H. Fan, Y. Lu, A. Stump, S. T. Reed, T. Baer, R. Schunk, V. Perez-Luna, Gabriel P. Lopez and C. J. Brinker, Nature, 405 (2000) 56. 22. A. Sayari, S. Hamoudi, Y. Yang, I. L. Moudrakovski and J. R. Ripmeester, Chem. Mater., 12 (2000) 3857. 23. S. Hamoudi, Y. Yang, I. L. Moudrakovski, S. Lang and A. Sayari, J. Phys. Chem. B, 105 (2001) 9118. 24. M. Kruk, M. Jaroniec, S. Guan and S. Inagaki, J. Phys. Chem. B, 105 (2001) 681. 25. C. H. Lee, S. S. Park, S. J. Choe and D. H. Park, Microporous Mesoporous Mater., 46 (2001) 257. 26. S. S. Park, C. H. Lee, J. H. Cheon and D. H. Park, J. Mater. Chem., 11 (2001) 3397. 27. K. Yamamoto, Y. Nohara and T. Tatsumi, Chem. Lett., (2001) 648. 28. M. C. Burleigh, M. A. Markowitz, M. S. Spector and B. P. Gaber, J. Phys. Chem. B, 105 (2001) 9935. 29. M. C. Burleigh, S. Dai, E. W. Hagaman and J. S. Lin, Chem. Mater., 13 (2001) 2537. 30. O. Muth, C. Schellbach and M. Fr6ba, Chem. Commun., (2001) 2032. 31. D. Ravaine, A. Seminel, Y. Charbouillot and M. Vincens, J. Non-Cryst. Solids, 82 (1986) 210. 32. B. Lintner, N. Arfsten, H. Dislich, H. Schmidt, G. Philipp and B. Seiferling, J. NonCryst. Solids, 100 (1988) 378. 33. J. D. Mackenzie, Y. J. Chung and Y. Hu. J. Non-Cryst. Solids, 147-148 (1992) 271. 34. D. A. Loy and K. J. Shea, Chem. Rev., 95 (1995) 1431. 35. J. J. E. Moreau and M. Wong Chi Man, Coord. Chem. Rev., 178-180 (1998) 1073. 36. M. A. Girtu, J. Opt. Adv. Mater., 3 (2001) 113. 37. R. J. P. Corriu, Angew. Chem. Int. Ed., 39 (2000) 1376. 38. H. W. Oviatt, K. J. Shea and J. H. Small, Chem. Mater., 5 (1993) 943. 39. G. Cerveau, R. J. P. Corriu and E. Framery, Chem. Commun., (1999) 2081. 40. D. A. Loy, G. M. Jamison, B. M. Baugher, E. M. Russick, R. A. Assink, S. Prabakar and K. J. Shea, J. Non-Cryst. Solids, 186 (1995) 44. 41. C. T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710. 42. J. S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T-W. Chu, D. H. Olson, E. W. Sheppard, S. B. McCullen, J. B. Higgins and J. L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. 43. T. Yanagisawa, T. Shimizu, K. Kuroda and C. Kato, Bull. Chem. Soc. Jpn., 63 (1990) 988. 44. S. Inagaki, Y. Fukushima and K. Kuroda, J. Chem. Soe., Chem. Commun., (1993) 680. 45. Q. Huo, D. I. Margolese, U. Ciesla, P. Feng, T. E. Gier, P. Sieger, R. Leon, P. M. Petroff, F. Schuth and G. D. Stucky, Nature, 368 (1994) 317. 46. P. T. Tanev and T. J. Pinnavaia, Science 267 (1995) 865.
26 47. 48. 49. 50.
S. A. Bagshaw, E. Prouzet and T. J. Pinnavaia, Science, 269 (1995) 1242. R. Ryoo, J. M. Kim, C. H. Ko and C. H. Shin, J. Phys. Chem. B, 100 (1996) 17718. Q. Huo, D. I. Margolese and G. D. Stucky, Chem. Mater., 8 (1996) 1147. D. Zhao, Q. Huo, J. Feng, B. F. Chmelka and G. D. Stucky, J. Am. Chem. Soc., 120 (1998) 6024. 51. Z.-R. Tian, W. Tong, J.-Y. Wang, N.-G. Duan, V. V. Krishnan and S. L. Suib, Science, 276 (1997) 926. 52. P. V. Braun, P. Osenar and S. I. Stupp, Nature, 380 (1996) 325. 53. D. M. Antonelli and J. Y. Ying, Angew. Chem. Int. Ed., 35 (1996) 426. 54. M. J. MacLachlan, N. Coombs and G. A. Ozin, Nature, 397 (1999) 681. 55. K. K. Rangan, S. J. L. Billinge, V. Petkov, J. Heising and M. G. Kanatzidis, Chem. Mater., 11 (1999) 2629. 56. M. J. MacLachlan, N. Coombs, R. L. Bedard, S. White, L. K. Thompson, G. A. Ozin, J. Am. Chem. Soc., 121 (1999) 12005. 57. G. S. Attard, C. G. Gtiltner, J. M. Corker, S. Henke, R. H. Templer, Angew. Chem. Int. Ed., 36 (1997) 1315. 58. D. Khushalani, A. Kuperman, G. A. Ozin, K. Tanaka, J. Garces, M. M. Olken and N. Coombs, Adv. Mater., 7 (1995) 842. 59. A. Sayari, M. Kruk, M. Jaroniec and I. L. Moudrakovski, Adv. Mater., 10 (1998) 1376. 60. G. A. Ozin, E. Chomski, D. Khushalani, M. J. MacLachlan, Curr. Opin. Colloid Interface Sci., 3 (1998) 181. 61. K. Moiler, T. Bein and R. X. Fischer, Chem. Mater., 10 (1998) 1841. 62. J. C. Vartulli, S. S. Shih, C. T. Kresge and J. S. Beck, Stud. Surf. Sci. Catal., 117 (1998) 13. 63. H. Hata, S. Saeki, T. Kimura, Y. Sugahara and K. Kuroda, Chem. Mater., 11 (1999) 1110. 64. D. Y. Zhao, P. D. u Q. S. Huo, B. F. Chemelka and G. D. Stucky, Curr. Opin. Solid State Mater. Sci., 3 (1998) 111. 65. M. H. Keefe, R. V. Slone, T. J. Hupp, K. F. Czaplewski, R. Q. Snurr and C. L. Stem, Langmuir, 16 (2000) 3964. 66. J. P. G. Pater, P. A. Jacobs and J. A. Martens, J. Catal., 184 (1999) 262. 67. C. E. Fowler, S. L. Burkett and S. Mann, Chem. Commun., (1997) 1769. 68. D. J. Maquarrie, Chem. Commun., (1996) 1961. 69. M. H. Lim, C. F. Blanford and A. Stein, Chem. Mater., 10 (1998) 467. 70. L. Mercier and T. J. Pinnavaia, Chem. Mater., 12 (2000) 188. 71. V. Antochshuk and M. Jaroniec, Chem. Commun., (1999) 2373. 72. R. J. P. Corriu, M. Granier and G. F. Lanneau, J. Organometal. Chem., 562 (1998) 79. 73. M. J. Kim and R. Ryoo, Chem. Mater., 11 (1999) 487. 74. C. A. Muller, M. Schneider, T. Mallat and A. Baiker, Appl. Catal. A, 201 (2000) 253. 75. D. Brunel, Microporous Mesoporous Mater. 27 (1999) 329. 76. D. J. Macquarrie, D. B. Jackson, S. Tailland, K. Wilson and J. H. Clark, Stud. Surf. Sci. Catal., 129 (2000) 275.
Studies in Surface Science and Catalysis 141 A. Sayariand M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rightsreserved.
27
Porous materials: L o o k i n g through the electron microscope O. Terasaki l*, T. Ohsuna2, Z. Liu 3, M. Kaneda l, S. Kamiya 1, A. Carlsson 1, T. Tsubakiyama 1, Y. Sakamot01, S. Inagaki 4, S. Che 5, T. Tatsumi 5, M. A. Camblor6, R. Ryoo 7, D. Zhao 8, G. Stucky9, D. Shindo 3 and K. Hiraga 2 1 Department of Physics and CIR, Tohoku University, Sendai 980-8578, Japan 2 Institute for Materials Research, Tohoku University, Sendai 980-8577, Japan 3 Insititute of Multidisciplinary Research for Advanced Materials, Tohoku University, Sendai 980-8577, Japan 4 Toyota Central R&D Laboratories, Inc., Nagakute, Aichi, 480-1192, Japan 5 Division of Materials Science & Chemical Engineering, Yokohama National University, Yokohama 240-8051, Japan 6 Industrias Quimicas del Ebro, Poligono de Malpica calle D, no 97, 50057 Zaragoza, Spain 7 Materials Chemistry Laboratory, School of Molecular Science-BK21, Korea Advanced Institute of Science and Technology, Taejon 305-701, Korea 8 Department of Chemistry, Fudan University, Shanghai 200433, P. R. China 9 Department of Chemistry & Biochemistry and Materials Department, University of California, Santa Barbara, California 93106, USA
Porous and confined materials with periodic micro and mesoscale pores have attracted much attention, both from fundamental and applied scientists. Increasingly, we are encountering new, structurally complex materials, whose structures cannot be solved/characterized by the usual methods available. Knowledge of their structures is essential for thorough understanding of their properties and further development. Therefore, the development of methods appropriate for structural analysis of these materials is a matter of urgency. Electron microscopy may be the best technique for this purpose, as long as we are interested in both local structures and average periodic structures. Here we describe general aspects of the structural analysis of periodic nanoporous materials and our latest achievements in this field.
*To whom correspondence should be addressed:
[email protected]
28 1. INTRODUCTION Porous crystals, both microporous (i.e., zeolites), and mesoporous, contain periodically arranged pores and cavities, from less than 20 A for microporous systems and between 20 and 500 A for mesoporous systems. They are of industrial use as molecular sieves for chemical separations, ion-exchangers for detergents, heterogeneous shape-selective catalysts, 16wdielectric materials and also as molds for synthesis of novel materials within their spaces. Knowledge of the structures of these crystals can provide important insights into their properties and can lead to the design of desirable materials. More than 130 different framework-type structures (zeolites) have been reported as microporous materials, and many new crystals remain unreported, because their structures have yet to be solved. Many ordered mesoporous silicas have also been synthesized using amphiphilic molecules as templates. They are not always a single phase, due to the kinetically controlled synthesis procedure. These porous crystals have the following obstacles, which make their structural analysis difficult: (i) Most as synthesized microporous materials are microcrystalline, with particle dimensions of 1 micron or less. They are thus too small for structural analysis by single-crystal X-ray diffraction (XRD) experiment. In the absence of single crystal data, the structural analysis and refinement must be carried out by powder XRD experiments. If the reflections in the powder XRD profile overlap significantly, solving the crystal structure from these data can be extremely difficult without reasonable initial structural models as zeolites may contain several hundred atoms in a unit cell. (ii) It is hard to determine even the crystal class of mesoporous solids uniquely by powder XRD, as only a few reflections (with large broadening) are observed in the XRD pattern. Furthermore, the mesoscale order is extremely sensitive to the synthesis conditions and mesoporous materials contain local structural fluctuations and sometime tend to form intergrowths. These obstacles can be overcome with HRTEM images obtained from thin regions coupled with digital Fourier analysis. The amplitudes and phases of crystal structure factors (CSFs) obtained from a set of HREM images can be used to solve the three-dimensional (3d) structures. Here, we will report our approach using electron crystallography (EC)[ 1,2,3,4].
2. CRYSTAL MORPHOLOGY OF MESOPOROUS MATERIALS Recently, mesoporous crystals have been synthesized under well-controlled conditions and display nice crystal morphologies [3,4,5]. However, local structural fluctuations in mesoporous materials are common and produce only a small number of reflections with large peak widths on the powder XRD patterns (we must observe XRD patterns more carefully with higher S/N ratio in order to observe reflections with weak intensity), even though the materials may show regular crystal morphology. This situation is illustrated in Figures 1 and 2, which show the SEM images and powder XRD patterns for cubic organic-inorganic hybrid [5], MCM-48 [6], SBA-1 [7] and 3d-hexagonal material [to be submitted]. All SEM images show very beautiful crystal morphologies, which are commensurate with the point group symmetries. However, it is difficult to determine crystal classes uniquely from the XRD patterns, although we can index all peaks in these patterns if we have definite information from other experiments or if we assume the crystal classes.
29
Figure 1. SEM images of (a)eubic hybrid, (b)MCM-48, (c)SBA-1 and (d)3d-hexagonal material.
(a)
i
U 201"
201"
(d)
(c)
i i
i f
/
/
1
20/~
20/"
Figure 2. XRD pattems of (a)hybrid material, (b)MCM-48, (c)SBA-1 and (d)3d-hexagonal material.
30 3. WHAT ARE THE ADVANTAGES OF ELECTRON CRYSTALLOGRAPHY? Using a CCD camera or imaging plate, we can now measure ED intensities or HREM image contrasts quantitatively over wide ranges in intensity, as they have larger dynamic range and better linearity of output to input electrons than photographic film. The advantages of using electrons as probes for structural study are: (i) electromagnetic lenses can be used for image formation and (ii) electrons interact with matter approximately 104 times stronger compared with X-rays. The latter feature allows us to use very small crystals, down to only several tens unit cells in size, to obtain single crystal structural information. A natural extension based on the latter is to collect electron diffraction intensity data from thin single crystals and then apply "direct methods" for phase recovery in CSFs. HREM images carry both phase and amplitude information of CSFs, and this is the most important advantage of using the electron crystallography (EC) for porous silicas, compared to the traditional single crystal X-ray diffraction. The phase is a most important parameter to build the crystal structure and we can apply weak phase object (WPO) approximation for samples up to a few hundreds A thick at 300 keV. The novel materials, which are synthesized within the pores of silica mesoporous crystals, sometimes show new hierarchical structures with order at both atomic and mesoscales [8,9]. We must develop an adequate method to solve/characterize the structure of these new materials because there is no such method yet.
4. OBSERVATIONS The samples were investigated with a JEM-3010 (operating at 300 kV, Cs=0.6 mm, structural resolution 1.7 A) and JEM-4000EX (operating at 400 kV, Cs=l.0 mm, structural resolution 1.7 A). Images were recorded with films and a CCD-camera (Model 794, Gatan, size 1024x1024, pixel size 25x25~tm 2) using low dose conditions. Diffraction patterns were also recorded using both films and the CCD-camera.
5. RESULTS AND DISCUSSION
5.1. Microporous Materials We can now measure ED intensities easily by using a CCD camera or imaging plate. Applying "direct methods" to the collected ED intensities of many independent reflections from different zone axes, we have been able to solve the previously unknown structure of zeolite SFE from a very small crystal [3]. The conditions for applying this method are carefully studied and they are dependent on the symmetry of crystals [T. Ohsuna et al., Annual Japanese Zeolite Association Meeting, 2000]. As zeolites have low density, kinematical treatment in diffraction is a good approximation for analysis of the ED intensity distribution, if specimens are thinner than a few hundreds A for 300 kV electrons. This is not a very difficult condition for zeolites if we can synthesize them as a single/pure phase. Since HRTEM images of zeolites have low resolution and only a few HRTEM images are available, a potential density map derived from Fourier reconstruction of the HRTEM images is usually blurred (low resolution). Hence, it is difficult to find atom positions in the potential map directly. We have introduced a new enhancement method for retrieving atom
31 positions and obtaining a reasonable framework structure from the blurred density map by using a Patterson map to give a vector connecting a pair of atoms. The map is obtained from electron diffraction intensity and is independent of the phases. Further refinement was carried out for T-atom positions together with O-atom positions using a similar technique as the DLS program. Whole procedure was carried out by a software package developed by one of the authors (TO) for the present problem. A new polytype of zeolite Beta, which is coded as BEC, was solved by this method [4, 10]. Two HREM images of BEC, taken with the [100] and [001] directions, were used for Fourier reconstruction. Figure 3 shows an HREM image of[100] incidence and the structure solution obtained is shown in Figure 4. The framework has three straight channels with 12-MRs window along [100], [010] and [001] directions, and the same stacking of BEC in HREM image of ITQ-14 can be seen as indicated by an arrow in Figure 5. Most of the image of Figure 5 is the same as that of ordinary Beta, which is mixture of polytype A and polytype B.
5.2. Mesoporous Materials We have developed a new method for solving the structure with mesoscale ordering without assuming any structural models based on electron crystallography, using the crystalline nature of 3d mesoporous materials. The resolution for the structure is primarily limited by the quality of the HREM images, which depends mostly on the long-range mesoscale ordering. Further progress may give better resolution and finer details will be obtained, however no change in conclusions will be necessary about the structure because the validity of a solution does not depend on the resolution. From observed images we can choose thin areas, which are free from dynamical scattering, and a large domain of a single phase from a multi-phase mixture. Figure 6 shows an HREM image of SBA-12 revealing domain structures, from which we could find a sufficiently large domain to solve a new 3dstructure, and this will be reported separately[ 10]. An HREM image of MCM-48 taken with [111] incidence and corresponding Fourier diffractogram, which is obtained from a thin region and clearly indicates extinction conditions for reflections, are shown in Figure 7a. From observations under extinction conditions from the diffractograms and the point group symmetry deduced from the morphology shown in Figure 2, the space group of MCM-48 was uniquely determined to be Ia 3d. Two dimensional (2d) data of CSFs were obtained from the images of each zone axis, and they were merged into a 3d-data set after normalizing by common reflections. The 3d-structure solution of MCM-48 was uniquely obtained from the 3d-data set of CSFs by inverse Fourier transformation, that is, Fourier Sum. The result shows that the amorphous wall-surface follows exactly the G-surface, one of periodic minimal surfaces, and the wall separates the structure into two enantiomeric channel systems, which are not interconnected with each other (Figures 8a and 8b). Other new 3d-structures of silica mesoporous crystals recently determined by EC will be presented at the meeting, together with structural time evolution, which might be related to "phase transition", for example, 2d-hex t o Pm 3n phase [Annual Japanese Physical Soc. Meeting, 2000 & 2001, to be submitted] or to Ia 3d phase. B
5.3. Novel Mesoporous Materials Once the 3d-structures of silica mesoporous crystals are solved, they are used as a template (or mold) for the synthesis of new nanostructured materials[8,9,12]. Carbon and Pt nanowirenetworks were synthesized within pores of silica MCM-48. Pores of MCM-48, both right and
32
!ool]
'~' ,~ [010] ~i~z,~!ii~iiii~ili~' ~~
Figure 3. HREM image of BEC [100]. "~'~ [010] [100]
Figure 4. Structure solution ofBEC [ 100].
!ii!iii!!! i. . ...... r. ii!9...!!iii!! i!!il ill ii
Figure 5. HREM image Of ITQ-14.
iliii!
9 ili
Figure 6. HREM image of SBA-12.
i i~
33
Figure 7(a). HREM image and Fourier diffractogram of MCM-48.
Figure 7(b). HREM image and Fourier diffractogram of Carbon network, CMK-4.
Figure 9. Pt nanowire-network.
Figure 8. The channel system of MCM-48.
34 left hand channel systems, are equally and uniformly filled by carbon, and therefore the images of MCM-48 and carbon network give reverse contrast (Figures 7a and 7b). Fourier diffractograms of the images give same diffraction patterns as expected from Babinet's principle. Pt-network was formed inside the channels of MCM-48 without destroying the channel geometry [8,9]. Figure 9 shows Pt nanowire-network when the incident beam is parallel to the [ 100] direction of MCM-48. Since the MCM-48 has a chiral channel structure, the Pt-networks formed inside such channels are also chiral[9].
6. CONCLUSIONS As shown here, we have overcome some obstacles and succeeded in obtaining the structure solutions of porous materials by the technique of electron microscopy, that is, EC. It was shown that Fourier reconstruction of the HREM image was powerful approach for the materials, and that recent improvement of synthesizing high quality crystals made it possible to solve the structures by EC. Once 3d-structure of porous crystals have obtained, we can use the crystals as mold/templates for the synthesis of novel advanced materials, which requires us new development for structure analysis appropriate to the new materials.
7. ACKNOWLEDGMENTS Financial supports from CREST, Japan Science and Technology Corp. (OT) and Creative Research Initiative Program (RR) are greatly acknowledged.
REFERENCES
1. A. Carlsson, M. Kaneda, Y. Sakamoto, O. Terasaki, R. Ryoo and H. Joo, J. Electron Microscopy, 48 (1999) 795. 2. Y. Sakamoto, M. Kaneda, O. Terasaki, D.Y. Zhao, J.M. Kim, G. Stucky, H.J. Shin and R. Ryoo, Nature, 408 (2000) 449. 3. P. Wagner, O. Terasaki, S. Ritsch, J. G. Nery, S.I. Zones, M.E. Davis and K. Hiraga, J. Phys. Chem. B, 103 (1999) 8245. 4. T. Ohsuna, Z. Liu, O. Terasaki, K. Hiraga and M. A. Camblor, submitted. 5. S. Inagaki, S. Guan, Y. Fukushima, T. Ohsuna and O. Terasaki, J. Am. Chem. Soc., 121 (1999) 9611, and 122 (2000) 5660. 6. M. Kaneda, T. Tsubakiyama, A. Carlsson, Y. Sakamoto, T. Ohsuna, O. Terasaki, S.H. Joo and R. Ryoo, J. Phys. Chem. B., in press. 7. S. Che, Y. Sakamoto, O. Terasaki and T. Tatsumi, Chem. Mater., 13 (2001) 2237. 8. H.J. Shin, R. Ryoo, Z. Liu and O. Terasaki, J. Am. Chem. Soc., 123 (2001) 1246. 9. O. Terasaki, Z. Liu, T. Ohsuna, H.J. Shin and R. Ryoo, Microsc. and Microanal., in press. 10. Z. Liu, T. Ohsuna, O. Terasaki, M.A. Camblor, M.J. Diaz-Cabafias and K. Hiraga, J. Am. Chem. Soc., 123 (2001) 5370. 11. Y.Sakamoto, I. Diaz, O.Terasaki, D.Zhao, JP. Pariente, JM Kim & GD. Stucky, submitted. 12. S. Jun, S.H. Joo, R. Ryoo, M. Kruk, M. Jaroniec, T. Ohsuna and O. Terasaki, J. Am. Chem. Soc., 122 (2000) 10712.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
Molecular imprinting enzymes
-
a
35
w a y to p r e p a r e effective m i m i c s o f natural a n t i b o d i e s a n d
Gfinter Wulff Institute of Organic and Macromolecular Chemistry Heinrich-Heine University Dfisseldorf, D-40225 Dfisseldorf, Germany
Molecular imprinting in synthetic polymers is used to prepare catalytically active imprinted polymers. Using different transition-state analogues of alkaline ester hydrolysis and suitable functional monomers, catalysts with strong esterolytic activity and enzyme-analogous properties are prepared. The polymers are obtained either as block polymers, and by standard suspension or mini-emulsion polymerization techniques. Through implementing the last two methods regular beads of 10 - 400 lam and minigels of 100 - 300 nm particle diameter are obtained. It is also possible to obtain soluble nanogels with diameters of 5 - 15 nm, i.e. in the same dimension as natural enzymes.
1. INTRODUTION The design of nano-scale specific arrangements in synthetic polymers can be obtained by an information transfer from low-molecular-weight compounds during the formation of the polymer. Thus the constitution and the configuration of complex arrangements in polymers can be controlled by specific interactions of the polymerizable monomers with a suitable template molecule. After polymerization of the monomer-template complex the original structure of the supramolecular arrangement will be stabilized and frozen. The removal of the template furnishes polymers with defined structures by transfer of structural information from the template to the polymer. If we look at the transfer of properties from the template to the resulting macromolecule, the situation is rather complicated since a large number of stereogenic centers are formed which are covalently linked with each other. Different possibilities exists: Through repetitive property transfer along a long chain it is possible to obtain structurally defined linear polymers which show a defined tacticity and in cases with optically active templates also optical activity (for reviews see [ 1, 2]). It is also possible to get an information transfer to a plain surface in a twodimensional manner (see [3, 4]). The case in which a crosslinking reaction is performed during the transfer is most interesting because a real three-dimensional transfer of properties (molecular imprinting) is possible in this instance. After removal of the template distinct cavities of a defined dimension of 0.5 - 2 nm, a predetermined shape, and an arrangement of functional groups in a predetermined stereochemistry can be obtained.
36 2. THE MOLECULAR IMPRINTING PROCEDURE
Scheme I Schematic representation of the molecular imprinting procedure [5]. Scheme I shows the principle of molecular imprinting, an approach we have introduced quite some years ago [5, 6]. Polymerizable vinyl monomers containing functional groups are attached to suitable template molecules(T) either by covalent or by non-covalent interaction. Subsequent copolymerization in the presence of solvent and large concentrations of crosslinking agent produces relatively rigid macroporous polymers. Removal of the template molecules (see Scheme I) leaves behind cavities in the polymer whose shape and whose arrangement of the
Scheme II Different types of interaction in the molecular imprinting technique.
37 functional groups are determined by the template molecules. The relation of template and imprint resembles very much the key-and-lock principle postulated for enzyme catalysis by Emil Fischer more than 100 years ago [7].
Scheme IIl Crosslinked polymers prepared from the template monomer 1 and removal of the template [6]. Template monomer 1 in Scheme II is shown as an illustration for covalent interaction, in which two molecules of 4-vinylphenylboronic acid have been bound to phenyl c~-Dmannopyranoside as the template by boronic ester linkages to the free hydroxyl groups. A 1 : 9 ratio of monomer 1 and ethylene dimethacrylate was copolymerized in an inert solvent to yield a macroporous polymer. From this the template could be split off to the extent of 9 0 - 95% providing chiral cavities each bearing a pair of boronic acid groups (Scheme Ill). Polymers of this type exhibit an excellent ability for racemic resolution of the racemate of the employed template. The original template enantiomer is preferably incorporated under batch equilibration and separation factors et (ratio of KD/KL) as high as 4 - 6 are achieved. These materials can also be used as chromatographic supports in h.p.l.c, columns giving resolutions higher than Rs = 4.3 (see Fig. 1) [8].
Gradient elution in h.p.l.c.: 70~ flow: l ml/min; gradient: acetonitrile incl. 5% aqueous NH3 (25%) and water incl. 5% aqueous NH3 (25%) 9:1 to 5:5
'
IfO
'
I 14
!
t / m i n -'-'-P
Figure 1
H.p.l.c. separation of the racemate of phenyl-c~-mannopyranoside on an adsorbent produced according to Scheme III.
38 These sorbents can be prepared conveniently and possess excellent thermomechanical stability. Even when used at 80~ under high pressure for a long period, no leakage of the stationary phase or decrease in selectivity during chromatography was observed [4]. Investigations as to the mechanism of this separation showed that the orientation of the functional groups within the cavities is the dominating factor for the separation; the shape of the cavity is of secondary importance [9]. In the meanwhile many other research groups all over the world have entered the field. Aside of covalent bonds as binding site interaction also metal-coordination has been used (for reviews see [10, 11] and Scheme II b). An interesting extension of the concept of molecular imprinting was introduced by Mosbach and his coworkers [12, 13] who used only non-covalent interactions during imprinting and the succeeding equilibration studies. In this case mostly hydrogen bonding and electrostatic interaction are used for the binding interaction (see Scheme IIc). A wide range of examples for different chemical classes of templates are known that have been used for molecular imprinting in crosslinked polymers. For general reviews on molecular imprinting see [books, 14, 15] and numerous review articles [4, 10, 13, 16-20]. Molecularly imprinted polymers have been used with great success as separation media (mostly in chromatography). Of special interest is the enantiomeric resolution of racemates. Further applications are as immunosorbents and chemosensors. The cavities in imprinted polymers have also been used as microreactors for selective reactions and, more interestingly, as the active sites of catalytically active polymers (see reviews [4, 10, 14-20]). In this paper the enzyme-like catalysis by molecularly imprinted polymers will be discussed as well as the influence of the state of dispersion on the catalytic activity. It is possible to obtain molecularly imprinted highly crosslinked microparticles in the order of 5 - 15 nm, i.e. in the same order of magnitude as natural enzymes, which are soluble in certain solvents.
3.
CATALYSIS WITH AMIDINE-CONTAINING MOLECULARLY IMPRINTED POLYMERS
Lemer et al. and Schultz et al. [21, 22] have shown that antibodies prepared against a stable transition state analogue of a reaction show considerable catalytic activity. Thus, antibodies prepared against a phosphonic ester (as a transition state analogue for alkaline ester hydrolysis) enhance the rate of ester hydrolysis 103 - 104 fold. Similarly, imprinting should also be an excellent method for preparing active sites of enzyme analogues. Various research groups have used this concept to prepare catalytically active polymers for ester hydrolysis, but their first results have been disappointing [23-25]. For a comprehensive review on catalytically active imprinted polymers see [26]. We have applied amidine functional groups for binding and catalysis. It was shown that N,N'-diethyl-4-vinyl benzamidine (2) is an advantageous binding site monomer for molecular imprinting since it shows a strong ionic, double bridged interaction between the amidine group and phosphonates, phosphates, and carboxylates [27, 28]. Phosphonic monoester 3 was used as the transition-state analogue for the alkaline ester hydrolysis [29]. The addition of two
39 equivalents of the binding site monomer 2 furnished a bisamidinium salt 4. By the usual polymerization, processing, and removal of the template, active sites were obtained with two amidine groups each. At pH 7.6 the imprinted polymer accelerated the rate of the hydrolysis of ester 5 more than 100 fold compared to the reaction in the same medium without polymer. In this case the formation of the diacid was measured. Was the released phenol measured instead a 235 fold acceleration was found. This shows that some product inhibition occurs. A polymer with statistically distributed amidine groups only showed a 20 fold acceleration.
% /OH __~ 0
EtN'~c\NHEt 2
caa ~ _
CH3
./," -- " ~',N
O
CH3 CH3
5
P\
\~N_H._67~
,,,,,,J
3
HOzC~ C \ o - - ~
-i*i O,~e~,O . ~ / c..
~N a -0
CH3 4
% ~,OH
o
o
Pho/P\oPh
Pho/C\oPh
Pho/C\NHPh
6
7
8
Further investigations showed that the molecularly imprinted polymers show typical enzyme analogue properties like Michaelis-Menten kinetics, competitive inhibition etc. From the obtained kinetic data a Michaelis constant, Km, of 0.60 mM, and a kcat of 0.8 " 10 -4 min ~ were obtained. The template molecule 3 is a powerful competitive inhibitor (Ki = 0.025 mM), which is bound more strongly than the substrate by a factor of 20. It is remarkable that such strong binding of the substrate and template occurs in water/acetonitrile (1:1). In order to avoid product inhibition the hydrolysis of carbonates and carbamates was investigated as well. Imprinted polymers were prepared from a complex obtained by addition of molar fractions of diphenylphosphate 6 and amidine 2. After the usual bulk polymerization the template 6 was removed and cavities with one amidine group each were obtained [30]. The hydrolysis of diphenylcarbonate 7 and diphenylcarbamate 8 was investigated in the presence of acetonitrile/buffer solution and in acetonitrile/buffer with the imprinted polymer. Substrate hydrolysis was treated as usual as a pseudo-first-order reaction and rate constants k of the initial reactions were determined. The ratio kimpr/ksol showed enhancements of 588 in the case of carbonate and 1400 - 3860 in the case of carbamate. The highest enhancements with respect to nonimprinted polymers containing statistically distributed amidine groups was 10 (carbonate) and 5.8 (carbamate) for these bulk polymers.
40 These values seem to be the highest accelerations published until now for molecularly imprinted catalysts. The activity for carbamate hydrolysis in this example is in the same order,of magnitude compared to catalytic antibodies [31]. In a similar fashion polymer catalysts were prepared for the hydrolysis of cholesterol carbonates [32].
4.
THE INFLUENCE OF THE TYPE OF DISPERSION ON THE CATALYTIC ACTIVITY
In the vast majority of cases, macroporous structures have been used for imprinted polymers. Macroporous polymers are obtained if polymerization of the monomers is carried out with a relatively high content of cross-linking agents (5 - 90%) in the presence of inert solvents (also known as porogens). During the polymerization phase separation takes plase and, after removal of the porogen and drying, a permanent pore structure remains. The relatively large inner surface area (50 - 600 m2g1) and large pores (about 10 - 60 nm) ensure that the specific microcavities formed by the imprinting process (between 0.5 - 2 nm in diameter depending on the template) are readily accessible and smaller molecules can diffuse freely inside the pores. If high levels of crosslinking agent are used, the cavities retain their shape quite well after removal of the templates.
a. Irregularly broken bulkpolymers, 5 - 500 ~tm, insoluble Figure 2
b. Spherical beads by suspension polymerisation, 2 - 500 lam, insoluble
c. Spherical beads by emulsion polymerisation, 100- 500 nm, insoluble
Different types of dispersion of molecularly imprinted polymers.
Usually the polymers are prepared in ampoules in the form of macroporous blocks which must then be crushed, ground, and sieved to obtain a desired particle size. Thus, irregularly broken bulk polymers with particle diameters of 5 - 500 I.tm can be obtained (see Fig. 2a). The preparation of these particles is a time consuming and energy-wasteful process. In addition, the properties of the resulting irregular particles may not be ideal with regard to flow, reproducibility, and scale-up procedures, whereas suspension polymerization methods produce relatively uniform spherical beads which are far more suitable (Fig. 2b). For these reasons, suspension polymerization has also been considered by others [33, 34], however, because of the used relatively weak interactions between the imprint substances and the binding site monomers in these cases simple suspension polymerization in water could not be applied. The new amidine monomer 2 allowed us to use the well-established suspension polymerization technique since the interaction between amidine and phosphonate, phosphate, or carboxylate is very stable.
41 Classical aqueous suspension polymerization techniques proceeded to smoothly give beads of 8 - 375 ~tm diameter, depending on the polymerization conditions used (e.g. mean diameter 31.3 ~tm; index of polydispersity of 1.16; surface area 277 m2/g; mean pore radius 6.3 nm, see also Table 1) [30]. The amidine-phosphate complex (from 2 and 6) or its components do not appear in the aqueous phase in the course of polymerization. The free, imprinted active sites were obtained by removal of the template. Table 1
Kinetic parameters for diphenyl carbonate hydrolysis with imprinted beads [30,36]
Particle size (index ofpolydisp.)
specific surface area (m2/g)
Hydrolysis of 7 relative reaction rate kimpr/ksol kimpr/kstat
Sample
porogen
water phase composition
SP 2
cyclohexanol/ dodecanol 9:1
20% NaC1 8% starch
375 ~tm (1.16)
288
168
24
SP 3
cyclohexanol/ dodecanol 9:1
0.2% PVP 0.1% PVA
31.3 ~tm (1.23)
234
150
23
M-1
-
2% PVP 1% PVA
149 nm
31
71
25
M-2
-
2% PVP 1% PVA
230 nm
20
54
17
The imprinted beads possess the same catalytic activity as bulk-type imprinted polymers if they are prepared with the same porogen, e.g., cyclohexanol-n-dodecanol (see Table 1). Although, the rate constants of diphenyl carbonate hydrolysis are apparently higher for polymers prepared on the basis of acetonitrile as porogen, it is impossible to use it in suspension polymerization due to the miscibility of acetonitrile with water. The enhancement with respect to non-imprinted polymers containing statistically distributed amidines is much higher with beads compared to bulk polymers. Enhancements of up to 24 are obtained. Thus, the beads show a much higher selectivity. It is also possible to obtain much smaller gel-type crosslinked minigels by emulsion polymerization by a method described first by Landvester et al. [35]. In this case no porogen is used and non-porous particles between 100 - 500 nm ~article diameter were obtained (minigels) (see Fig. 2c). The surface area is smaller (15 - 35 m / g ) since there is nearly no inner surface area present. These particles are insoluble in all solvents used but in some cases they can be solubilized in colloidal form. The same chemical composition as used with bulk polymerization and suspension polymerization was used in this case with the exception that no porogen was present (see Table 1) [36]. Although, the polymers prepared by suspension polymerization had much higher surface areas compared to the minigels (around 10 fold), the observed rate enhancements kimpr/ksol are only reduced by 1/3 to 1/2 and the kimpr/kstat are in the same order of magnitude (see Table 1).
42 Even more interesting would be the synthesis of imprinted microgels. Microgels are defined in polymer chemistry as unimolecular, crosslinked polymer particles possessing a size comparable to the statistical dimensions of noncrosslinked macromolecules (5 - 15 nm) which can exist as stable solutions in appropriate solvents. It should be possible to introduce into these microgels (or nanogels) imprinted cavities obtaining soluble particles with dimensions comparable to those of enzymes (see Fig. 3a and b). For this reason we have systematically investigated the synthesis of highly crosslinked, molecularly imprinted microgels [37].
a. Natural enzymes, e.g. chymotrypsin =:> radius of gyration 5- 15nm molecular weight 30000 - 500000 =:> soluble
Figure 3
b. Intramolecularly crosslinked macromolecules (nanogels, microgels) =:>radius of gyration of less than 15 nm in solution molecular weight 50000 - 200000 =:> soluble
c. Macrogels obtained by usual crosslinking polymerisation Three-dimensional infinite network insoluble
lntramolecularly crosslinked macromolecules.
The problem in this synthesis is that usually under these conditions under intermolecular crosslinking three-dimensional infinite networks of macrogels are obtained (Fig. 3c). In special solvents (e.g. cyclopentanone) at low monomer concentration (e.g. 1%) it is possible to obtain highly crosslinked (nominal degree of 70%) soluble microgels with molecular imprinting. They were characterized through GPC, viscosimetry, and membrane osmometry, and were found to be highly crosslinked macromolecules with a molecular weight comparable to the one of proteins (see Table 2). Molecular recognition experiments clearly pointed out the presence of selective functionalized cavities within the microgels. Recognition experiments can be performed in homogeneous solution, after which the microgels are conveniently separated by ultracentrifugation or by precipitation. At present experiments are undertaken with transition state analogue imprinted soluble microgels which are imprinted with a complex of 6 and 2 and which are catalytically active in hydrolyzing the diphenylcarbonate (7) [38].
43 Table 2
Synthesis and characterization of molecularly imprinted nanogels [37]
Solvent
% yield Mw Mn Mw/M. Mn(osm) q a-value monomer % mixture Cyclopentanone 1 88 4 . 0 104 9 . 2 103 4.3 3.5 " 10~ 7.9 1.1 Cyclopentanone 2 91 5.1 " 105 2 . 2 104 23 n.d. 11.8 1.2 Cyclopentanone 3 92 Partially gelated nld. 1.4 DMF 1 76 4.2104 1.2104 3.4 4.9105 5.5 1.2 ACN/toluene 1:1 1 85 8.5 " 104 1.3 " 104 6.8 7 . 0 105 n.d. n.d. Monomer mixture consisting of 70% ethylene dimethacrylate, 25% methyl methacrylate, and 5% monomer 1. Radically initiated polymerisation ( AIBN ) at 80~ for 4 days. Mw = weight averaged- Mn = number averaged molecular weight from GPC. Mn(osm) = membrane osmometry; r I = intrinsic viscosity; a-value = equilibratio of the microgel after template removal with the racemate of phenyl a-mannopyranoside. Mimicking natural enzyme action is quite a demanding task. Molecular imprinting has brought quite some progress in this direction. Typical enzyme properties like Michaelis-Menten kinetics, competitive inhibition, induced fit etc. were observed. The catalytic activity of natural enzymes, though, is much higher by several orders of magnitude but the catalysts obtained are rather stable and can be easily prepared. Soluble nanogels in which each particle possesses one active site will be of special interest since enzyme analogy will be relatively high in this case.
5. ACKNOWLEDGEMENT This work was supported by Deutsche Forschungsgemeinschafi and Fonds der Chemischen lndustrie.
REFERENCES
[1] [2]
G. Wulff, Angew. Chem. 101 (1989) 22; Angew. Chem. Int. Ed. Engl., 28 (1989) 21. G. Wulff, in: A. D. Schliiter, Ed., Synthesis of Polymers, Wiley-VCH Verlag, Weinheim, 1998, pp. 375-401. [3] G. Wulff, B. Heide, G. Helfmeier, J. Am. Chem. Soc. 108 (1986) 1089. [4] G. Wulff, Angew. Chem. 107 (1995) 1959; Angew. Chem. Int. Ed. Engl. 34 (1995) 1812. [5] G. Wulff, A. Sarhan, K. Zabrocki, Tetrahedron Lett. (1973) 4329. [6] G. Wulff, W. Vesper, R. Grobe-Einsler, A. Sarhan, Makromol. Chem. 178 (1977) 2799. [7] E. Fischer, Ber. Dtsch. Chem. Ges. 27 (1894) 2985. [8] G. Wulff, M. Minarik, J. Liquid Chromatogr. 13 (1990) 2987. [9] G. Wulff, S. Schauhoff, J. Org. Chem. 56 (1991) 395. [10] S. Mallik, S. D. PlunkeR, P. K. Dhal, P. D. Johnson, D. Pack, D. Shnek, F. H. Amold, New J. Chem. 18 (1994) 299.
44 [ 11] P.K. Dhal, in: B. Sellergren, Ed., Molecularly Imprinted Polymers - Man Made Mimics of Antibodies and Their Application in Analytical Chemistry, Elsevier, Amsterdam, 2001, pp. 185-201. [12] B. Sellergren, M. Lepist6, K. Mosbach, J. Am. Chem. Soc. 110 (1988) 5853. [ 13] K. Mosbach, O. Ramstr6m, Biotechnology 14 (1996) 163. [ 14] R.A. Bartsch, M. Maeda, Eds., Molecular and Ionic Recognition with Imprinted Polymers, ACS Symposium Series, Vol. 703, Washington, 1998. [15] B. Sellergren, Ed., Molecularly Imprinted Polymers. Man-Made Mimics of Antibodies and Their Application in Analytical Chemistry, Elsevier, Amsterdam, 2001. [ 16] G. Wulff, in: F. Diederich, P. J. Stang, Eds., Templated Organic Synthesis, Wiley-VCH, Weinheim, 1999, pp. 3 9 - 73. [17] K. Mosbach, Trends Biochem. Sci. 19 (1994) 9. [ 18] K.J. Shea, Trends Polym. Sci. 2 (1994) 166. [19] T. Takeuchi, J. Matsui, Acta Polym. 47 (1996) 471. [20] M.J. Whitcombe, E. N. Vulfson, Adv. Mater. 13 (2001) 467. [21] R.A. Lerner, S. J. Benkovic, P. G. Schultz, Science 252 (1991) 659. [22] P. G. Schultz, Angew. Chem. 101 (1989) 1336; Angew. Chem. Int. Ed. Engl. 28 (1989) 1283. [23] D. Robinson, K. Mosbach, J. Chem. Soc., Chem. Commun. (1989) 969. [24] B. Sellergren, K. J. Shea, Tetrahedron Asymmetry 5 (1994) 1403; B. Sellergren, R. N. Karmalkar, K. J. Shea, J. Org. Chem. 65 (2000) 4009. [25] K. Ohkubo, K. Sawakuma, T. Sagawa, J. Mol. Cat. A 165 (2001) 1; and earlier papers of this group. [26] G. Wulff, Chem. Rev. in press. [27] G. Wulff, A. Biffis, in: [ 15], pp. 71 - 111. [28] G. Wulff, K. Knorr, Bioseparation, in press. [29] G. Wulff, T. Gross, R. Sch6nfeld, Angew. Chem. 109 (1997) 2049; Angew. Chem. Int. Ed. Engl. 36 (1997) 1961. [30] A.G. Strikowski, D. Kasper, M. Grfin, B. S. Green, J. Hradil, G. Wulff, J. Am. Chem. Soc. 122 (2000) 6295. [31] P. Wentworth, A. Datta, S. Smith, A. Marshall, L. J. Partridge, G. M. Blackburn, J. Am. Chem'. Soc. 119 (1997) 2315. [32] J.-M. Kim, K.-D. Ahn, G. Wulff, Macromol. Chem. Phys. 202 (2001) 1105. [33] K. Hosoya, K. Yoshizako, N. Tanaka, K. Kimata, T. Araki, J. Haginaka, Chem. Lett. (1994) 1437. [34] L. Ye, P. A. G. Cormack, K. Mosbach, Anal. Commun. 36 (1999) 35. [35] K. Landvester, N. Bechthold, F. Tiarks, M. Antonietti, Macromolecules 32 (1999) 2679. [36] A. Strikowski, B. S. Green, G. Wulff, unpublished results. [37] A. Biffis, N. B. Graham, G. Siedlaczek, S. Stalberg, G. Wulff, Macromol. Chem. Phys. 202 (2001) 163. [38] B.-O. Chong, G. Wulff, unpublished results.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
45
Plugged Hexagonal Mesoporous Templated Silica: A unique micro- and mesoporous material with internal silica nanocapsules. P. Van D e r Voort a'! , P. I. Ravikovitch b, A.V. Neimark b, M. Benjelloun a, E. Van Bavel a, K.P. De Jong c, B. M. Weckhuysen c and E.F. Vansant a. a University of Antwerp (UIA), Dept. of Chemistry, Universiteitsplein 1, B-2610 Wilrijk, Belgium. i Corresponding author; email
[email protected]
b Center for Modeling and Characterization of Nanoporous Materials, TRI Princeton, P.O. Box 625, Princeton, NJ 08542, USA. $cUniversity of Utrecht, Dept. of Inorganic Chemistry and Catalysis, Debye Institute, Sorbonnelaan 16, 3508 TB Utrecht, The Netherlands. Following the development of purely mesoporous templated silicas, it is a desirable next step to create innovative catalytic support materials, consisting of a stable composite matrix with combined micro- and mesoporosities and a sufficient stability to withstand most industrial treatments. We show in this paper the development of a hexagonal plugged material, with combined micro- and mesopores and a tunable amount of both open and inkbottle mesopores. The ratios of these different pore types are variable in a wide range. The obtained materials are much more stable than the conventional micellar templated structures known so far. 1.
INTRODUCTION
Following the pioneering publications on the synthesis of mesoporous, semi-crystalline silicas [1-4], intensive research efforts have been devoted to the development of new mesoporous support materials of ordered structure. The research is motivated by the fact that such materials fill the gap in catalytic chemistry between the crystalline microporous zeolites and amorphous, disordered mesoporous supports like silica gel [5]. Due to their controlled pore size and a very narrow pore size distribution, the ordered mesoporous materials have a large potential as catalytic support in fine chemistry [5], pharmaceutical industry [7], as well as for the production of special polymer materials [6]. Heterogenizing the synthetic procedures in these fields of chemistry forms an important tool in achieving the goals of green, sustainable production processes and end-of-pipe waste reduction [7]. It is desirable to create innovative catalytic support materials, consisting of a stable composite matrix with combined micro- and mesoporosities. Such materials will offer significant supplementary advantages of an improved diffusion rate for transport in catalytic processes (faster reactions); better hydrothermal stability [8]; synthesis of multifunctional catalysts, which can process a large variety of feedstocks; capabilities of encapsulated waste in the micropores; controlled leaching rates for a constant and gradual release of an active component, etc. Here, we present a very simple synthesis procedure of a plugged hexagonal mesoporous material with very thick walls, high stability and controllable and tunable micro- and mesoporosities.
46 2.
EXPERIMENTAL
A plugged MTS material is prepared by dissolving 4 g of Pluronic P123 (non-ionic triblock copolymer, EO20POToEO20)in an acidic water/HC1 solution. Subsequently, an amount of TEOS (between 5 and 25 g) is added. The solution is stirred for 4-8 hours at a fixed temperature between 40 and 80~ and subsequently aged at ambient pressure for 17 h at 80120~ The white solid was filtered, washed and calcined at 550~ Detailed experimental conditions can be found in [9]. X-Ray Diffractograms were recorded on a Philips PW1840 powder diffractometer, using Ni-filtered Cu Ka radiation. Porosity and surface area studies were performed on a Quantachrome Autosorb-1-MP automated gas adsorption system. The calcined samples were degassed for 17 h at 200~ TGA measurements were recorded on a Mettler TG50 thermobalance. Mechanical pressing tests were performed in a unilateral press with a typical 13 mm dye (Specac). Hydrothermal tests were performed by placing the sample on a grid in an autoclave, which is filled with liquid water underneath the grid. The entire system is placed in an oven for 17 h in the temperature range 120-160~ exposing the sample to steam at autogeneous pressure. Other hydtrothermal experiments were performed using a fixed bed reactor, using a nitrogen flow, saturated with a certain percentage of water vapor.
3. RESULTS AND DISCUSSION
3.1. Nitrogen isotherms Changing the synthesis parameters in a controlled way allows the reproducible synthesis of a broad variety of materials. The adsorption-desorption isotherms of three distinctly different materials are shown in Figure 1. The isotherm in figure 1A is typical for the SBA-15 material [3], a two-dimensional p6mm structure formed by open cylindrical mesopores > ca. 5 nm in diameter. The desorption isotherm corresponds to the vapor pressure of the equilibrium meniscus in the open cylincrical pore, while the adsorption isotherm corresponds to the limit of stability of the adsorption film [ 10]. It should be noted that the material contains significant amounts (up to 30% of the porosity) of intrawall micropores (< ca. 3 nm) located in the pore walls, as evaluated by the NLDFT method [11]. The isotherm in Figure 1C shows the isotherm of a material with regular cylindrical pores that are accessible only through permeable microporous plugs. This is evident from the desorption branch of the isotherm and the shape of the hysteresis loop. If a pore is plugged, desorption is delayed until the vapor pressure is reduced below the desorption pressure from a pore aperture (ink-bottle efffect). However, if the pore aperture is below a critical diameter, decrease in the vapor pressure causes the fluid in the larger pores to become thermodynamically unstable before the desorption pressure for the pore aperture is reached [ 12]. For nitrogen at 77 K this instability occurs at p/p0: 0.42-0.45. The isotherm in Figure 1B is remarkable. It exhibits the following characteristic features: 1) adsorption in intrawall micropores at low relative pressures; 2) multilayer adsorption in regular mesopores and capillary condensation in narrow intrawall mesopores; 3) a one-step capillary condensation, indicating uniform mesopores; 4) a two-step desorption branch indicating the pore blocking effects (sub-step at the relative pressure of ca. 0.45). The adsorption-desorption behavior is consistent with a structure comprising both open and closed cylindrical mesopores. This interpretation is fully supported by the non-local density functional theory (NLDFT) of adsorption and hysteresis in cylindrical pores [ 10]. The mesopore size distribution and the total amount of micropores are calculated from the
47 adsorption branch of the isotherm by the NLDFT method [11]. The fractions of open and closed mesopores, as indicated schematically in Figure 2, have been determined from the pore size distributions (see Table 1). Details of calculations will be presented elsewhere.
Figure I : Nitrogen adsorption-desorption isotherms of (A) SBA-15, all open mesopores, (B) plugged material, with combined open and closed mesopores and (C) material with exclusively closed mesopores.
Figure 2. Nitrogen adsorption-desorption isotherm (77K) of a plugged hexagonal mesoporous templated silica and the mesopore size distribution calculated by the NLDFT method [ 10].
48 3.2. X-Ray Diffractogram The X-Ray Diffraction pattem in Figure 3 shows the characteristic reflections for a 2D hexagonal pore ordering in the p6mm space group [3]. The plugged mesoporous material therefore has the same structure as the SBA-15 hexagonal material.
Figure 3 : X-Ray Diffractogram of the plugged hexagonal mesoporous silica sample.
3.3. Plugged hexagonal mesoporous templated silica The data in Figures 1-3 point towards a composite material with a combined micro- and mesoporosity, as schematically represented in Figure 4. The rather thick walls ( - 4 nm) of the large cylindrical mesopores are perforated with micropores. Moreover, the cylindrical mesopores themselves are 'plugged' with amorphous silica nanocapsules, which are also microporous. These nanocapsules are created by large excess of the silica source (TEOS) that is used in the synthesis and by rapid hydrolysis of the silicon alkoxide at the very low pH used in the synthesis. The micropores in the silica walls can be explained by the penetration of hydrophilic poly(ethyleneoxide) chains of the triblock copolymer in the silica wall, as already suggested by Kruk et al [13]. The microporosity of the plugs may have a different origin. It is known that Pluronic triblock copolymers are in fact polydisperse mixtures of several triblock copolymers with a wide range of molecular weights, and that they contain appreciable amounts of diblock copolymers and even free PO chains. Some of these components, especially the low molecular weight ones, may not be involved in the actual templating of the mesopores, but still act as templates for the disordered nanocapsules, inducing a complementary porosity. The mesopores themselves are created by the so-called charge compensating templating mechanism of the entire triblock copolymer. The most important characteristics of these materials are summarized in Table 1. The table evidences the large variety in sample characteristics that can be obtained. The thickness of the mesoporous walls is typically 3-4 nm, which is excellent, compared to a typical wall thickness of 1 nm for the well-known MCM-41 structure. Extremely high total pore volumes can be obtained. The contribution of micropores (with contributions of both micropores in the walls and micropores in the silica nanocapsules) has an unprecedented high value. Micropore volumes up to 0.3 cm3/g can be obtained (40% of the total pore volume), which is
49 considerably higher than the micropore volumes of any composite material known so far. Both the ratio micropore/mesopore volume as the ratio open/closed mesopores is tunable in a wide range.
Microporous pore wall Microporous silica plugs 9
9
./ 9
9
............. 9...................................
......
9
9
9...... 9...............
9 9 ................................ 9
9
9 9
9
9
9
9
~
.
_
9
:l
6-8 nm
~ 1 7 96
9
3-4 nm
9
Open mesopore Closed mesopore Figure 4 9Schematical representation of the plugged hexagonal mesoporous templated silica (PHMTS) Table 1" Structural characteristics of 4 selected samples, PHMTS : Plugged Hexagonal Mesoporous Templated Silica, a0- lattice spacing, Vtot- totfil pore volume (micropores and mesopores), gmi- micropore volume, Vine- mesopore volume, Dads-- pore diameter from the adsorption branch, Does- - pore diameter from the desorption branch, Dgeom-- pore diameter from geometrical considerations using Vm,, Vine and 2.2 g/cm 3 for the silica skeleton density, hw pore wall thickness, hw = a0 - Daos; Vine(open)- volume of open mesopores, Vine (closed)volume of closed mesopores Sample
a0
(nm) SBA-15
ll.31
PHMTS-1
Vtot
SBET
Vmi
Vine
Dads
Ddes
Dg.... hw (ads) Vme(open) Vme (closed)
(cm3/g) (mVg)(cm3/g)(cm3/g)(nm)
(nm) (nm)
1.25
(nm)
(cm3/g)
(cm3/g)
950
0.14
l.ll
7.3.
7.59
7.76
4.01
l.ll
0
I 1.08 1.03
1040
0.29
0.74
6.79
7 . 0 3 7.12
4.30
0.23
0.51
PHMTS-2
9.58
0.71
880
0.26
0.45
6.08
no
5.89
3.50
< 0.01
0.45
PHMTS-3
10.16 0.83
945
0.30
0.53
7.03 7.03
6.94
3.13
0.38
0.15
.........
50
3.4. Transmission electron microscopy Using a Philips CM200 microscope, we have investigated extensively the PHMTS and SBA-15 samples in bright field transmission mode. In figure 5 we show representative images for these materials. Both micrographs provide side-on views of the ordered mesopore system. While"the mesopores in SBA-15 run smoothly over several micrometers of length, the PHMTS displays smaller domain sizes for the ordered mesopores. Moreover, the wall thickness yaries more strongly for the latter material, which may be caused by the presence of silica plugs inside the mesopores. Most recently, 3D-TEM techniques have been developed to image mesopores in three dimensions [14,15]. In a future paper, we will present evidence from 3D-TEM for the different pore systems in SBA-15 and our novel material PHMTS [9].
Figure 5" TEM images of SBA-15 (left) and PHMTS (fight).
3.5.
Stability
Table 3 presents the intrinsic thermal, mechanical ~and hydrothermal stabilities of some of the most important MTS materials [16]. Table 3 reveals that all materials are poorly resistant to (mild) hydrothermal treatments. The SBA-15 is the best. resistant of the conventional mesoporous silicas ; the PHMTS material is by far the most stable. It still has a very significant surface area and pore volume after 5 days of hydrothermal treatment or after a 24 h treatment in an autoclave in pure steam (sample placed above the water on a grid). Most materials collapse after a thermal treatment at 750~ with two exceptions: MCM-41 and PHMTS. Resistance toward mechanical (unilaterial) pressure is again best for PHMTS, followed by SBA-15. The thick walls of SBA-15 are further stabilized and supported in the PHMTS structure by the silica plugs, resulting in an extremely high mechanical resistance. The reported 10 tons/13 mm 2 was the highest pressure that could be obtained in our press. Pure silica based materials are obviously stable in neutral and acid conditions, but decompose in alkaline conditions.
51
Table 3 : Intrinsic stabilities of MTS materials ; SA = surface area (mZ/g), PV = pore volume (ml/g). Thermal stabilities after treatment in furnace, ambient atmosphere for 17 h at indicated temperature. Hydrothermal stability at x% water vapour at y temperature for z hours of treatment. Mechanical pressure, structure is collapsed if the XRD peak < 25% of the original peak and / or the typical diffraction peaks are no longer present. Chemical resistance : stirring for 24 h in an aqueous solution with indicated pH. l. Pressures are expressed as tons per 13 mm 2 pellet ; 1 ton/13 mm 2 corresponds to 740 bar. Treatment
MCM- 41 [PV SA
Themaal T :550~ 1027 T :650~ 970 T :750~ 879 T :850~ 795 Hydrothermal 25%/400/50 892 25%/400/120 864 100%/100/24 106 Mechanical 25% pressure I "ftonsI Chemical pH= 1 + pH = 7 + pH= 13 .
MCM- 48 [PV SA
HMS SA [ PV
SBA- 15 SA I PV
0.90 0.76 0.68 0.53
1433 1248 108 -
1.14 0.73 <0.05
1021 957 213 . .
0.81 718 0.58 561 <0.05 63 . .
0.66 0.59 <0.05
1357 1318 197
1.00 0.93 <0.05
915 830 228
0.57 0.48 <0.05
[ 4 tons
[ 5 tons
+ + .
+ + .
533 445 281
,PHMTS : [S~ :[)~
0.72 9!3::i i t 0!86 0.63 667 :: I 0.66 <0.05 451 0i48 !387 '~0~39 i 71:11' ::' ': : " " ...... : I 0.57 , 0.49 [~8~:: 1.0.47
~:!lOi~i I ~'
I 8 tons + +
.
4. C O N C L U S I O N S Using triblock copolymers as surfactant and TEOS as the silicon source, a whole variety of materials can be prepared, varying from pure SBA-15 (hexagonal stacking of pores, all pores are open) to hexagonal systems with exclusively ink-bottle pores and materials with combined open and closed pores, referred to as PHMTS (Plugged hexagonal mesoporous templated silica). PHMTS is characterized by very large but narrow distributed pores with very thick and microporous pore walls. Moreover, the pores are plugged internally with microporous silica nanocapsules. Their stability (thermal, hydrothermal, mechanical) is extremely high, compared to other commonly used mesoporous silicas. These materials might have unprecendented applications as adsorbers, desorbers and catalytic supports.
Acknowledgements This research was funded by a grant from the University of Antwerp (Special Research Fund) and by the F.W.O. (Flemish Fund for Scientific Research). The authors are grateful to Mrs. Sandra Kemp for making the TEM images.
5. REFERENCES 1. C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli and J.S. Beck, Nature 359 (1992) 710. 2. P.T. Tanev, M. Chibwe and T.J. Pinnavaia, Nature 368 (1994) 321; P.T. Tanev and T.J. Pinnavaia, Science 267 (1995) 865.
52 3. D. Zhao, J. Feng, Q. Huo, N. Melosh, G.H. Fredrickson, B. Chmelka and G.D. Stucky, Science 279 (1998) 548; D. Zhao, Q. Huo, J. Feng, B. Chmelka and G.D. Stucky, J. Am. Chem. Soc. 120 (1998) 6024. 4. S.A. Bagshaw, E. Prouzet and T.J. Pinnavaia, Science 269 (1995) 1242. 5. A. Corma, Chemical Reviews 97 (1997) 2373. 6. B.M. Weckhuysen, R.R. Rao, J. Pelgrims, R.A. Schoonheydt, P. Bodart, G. Debras, O. Collart, P. Van Der Voort and E.F. Vansant, Chemistry A European Journal 6 (2000) 2960. 7. J.H. Clark, Green Chemistry 1 (1999) 1. 8. A. Karlsson, M. St6cker and R. Schmidt, Microp. and Mesop. Mater. 27 (1999) 181. 9. P. Van Der Voort, P. I. Ravikovitch, A.V. Neimark, M. Benjelloun, E. Van Bavel, K.P. De Jong, A.H. Janssen, B. M. Weckhuysen and E.F. Vansant, in preparation. 10. A.V. Neimark, P.I. Ravikovitch and A. Vishnyakov, Phys. Rev. E 62 (2000) R1493. 11. P.I. Ravikovitch and A.V. Neimark, J. Phys. Chem. B 105 (200.1) 6817. 12. P.I. Ravikovitch and A.V. Neimark, Langmuir, submitted. 13. M. Kruk, M. Jaroniec, C.H. Ko and R. Ryoo, Chem. Mater. 12 (2000) 1961. 14. A.J. Koster, U. Ziese, A.J. Verkleij, A.H. Janssen and K.P. De Jong, J. Phys. Chem. B 104 (2000) 9368. 15. A.H. Janssen, A.J. Koster and K.P. De Jong, Angew. Chem. Int. Ed. 40 (2001) 1102. 16. K. Cassiers, T. Linssen, M. Mathieu, M. Benjelloun, P. Van Der Voort, P. Cool and E.F. Vansant, Chem. Mater., in press.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
I m p r i n t i n g o f the surface directing agents
of mesoporous
53
silicates u s i n g
organic
structure
Kaveri R. Sawant and Raul F. Lobo Center for Catalytic Science and Technology, Department of Chemical Engineering, University of Delaware, Newark, Delaware 19716, USA
A new protocol has been developed for incorporating the tetrapropylammonium cation (TPA +) into the walls of the mesoporous material SBA-15 with subsequent calcination to form a novel porous material. This modified material has been extensively characterized using powder x-ray diffraction (PXRD), nitrogen sorption studies, NMR spectroscopy, thermogravimetric analyses (TGA), SEM and TEM. As a'result of this treatment, the original mesoporous structure of SBA-15 is retained with a slight decrease in the unit cell dimension from 107 to 105 A. The average pore diameter is increased from 48 to 68 A although the total pore volume remains the same. 29Si MAS NMR spectra indicate that the silica phase is further condensed and densified. As a result a concomitant loss in BET surface area from 770 to 390 m2/g is observed. The incorporation ofTPA + into the amorphous siliceous walls of SBA-15 is confirmed by 13C-{1H} CP MAS NMR spectroscopy and by TGA. 1. INTRODUCTION The M41S family [1] and the related SBA-15 [2] mesoporous materials are a class of ordered porous silicates with pore diameters in the range of 20-500 A (see review [3]). Despite their large pore dimensions compared to that of zeolites, mesoporous materials are restricted in their use as catalysts for large organic molecules by their poor thermal stability and broad distribution of acid sites. A combination of the large pore dimensions of mesoporous materials with the strong acid sites present in zeolite-like structures would be highly advantageous leading to a novel and probably useful catalytic material. Hydrocarbon reactions involving large organic molecules that cannot enter the small pores of a zeolite catalyst may be catalyzed by the new material having a mesoporous framework structure with accessible strong acid sites on the surface of these large pores. Various strategies have been reported in the literature to combine some of the features of different porous materials [4-8]. Partial "recrystallization" of the surface of MCM-41 resulted in a mesoporous material with surface-tectosilicate structures giving enhanced acidity and catalytic cracking activity [4]. However, the walls of MCM-41 have a thickness of - 10 A and can contain, at most, very small organized units of silica/alumina. A dual templating method has been used for the synthesis of macroporous silicates with zeolitic microporous frameworks [5] and MCM-41/ZSM-5 composites [6]. In addition, another technique for the synthesis of macroporous materials with zeolitic microporous frameworks by self-assembly
54 of colloidal zeolites has been reported [7]. Finally, to obtain a mesoporous material with acid sites on the 'surface, a procedure has been reported for the syntheses of organically functionalized mesoporous materials with sulfonic acid groups [8]. This study reports a new protocol that has been developed for the synthesis of a novel mesoporous silicate that is obtained by reorganizing the structure of the walls of the mesoporous material SBA-15. SBA-15 is an all-silica mesoporous material consisting of long cylindrical pores ordered in a hexagonal packing arrangement with pore diameters in the range of 46-100 A [2]. The wall thickness is in the range of 31-64 ,~. The amorphous silica phase is itself structured and contains fine microporous channels interconnecting the large mesopores [10-11]. The use of a mesoporous precursor such as SBA-15 with a relatively large wall thickness o f - 59/k would allow structures comparable in size to the unit cells of zeolites like silicalite-1 thus increasing stability and catalytic activity. TPA + which serves as the organic structure directing agent (SDA) for the zeolite silicalite-1 was used to "imprint" silicalite-l-like domains within the thick amorphous pore walls of the mesoporous material SBA-15. Glycerol is used as a solvent, which also helps in the recrystallization of the silica phase. After the treatment the TPA + containing samples are calcined to remove the organic and obtain the porous novel material. These treated samples before and after calcination are referred to as TPA+-SBA - 15 and TPA+-SBA - 15 calcined respectively (Figure 1).
N
N
N
Amorphous Silica Phase SBA-15 (a)
O = TPA + ~
TPA+_SBA_I 5 (b)
Organized Silica Structure TPA+-SBA - 15 calcined (c)
Figure 1. Synthesis Strategy: (a) SBA-15 is treated with TPAOH and glycerol to obtain (b) the new material containing the incorporated TPA + (TPA+-SBA-15) which is then calcined to remove the TPA + to obtain (c) the final porous material (TPA+-SBA - 15 calcined). As a result of this treatment, the original mesoporous structure of SBA-15 is retained with a slight decrease in the unit cell dimension from 107 to 105 ,~. The average pore diameter is increased from 48 to 68 ~ although the total pore volume remains the same. 29Si MAS NMR spectra indicate that the silica phase is further condensed and densified as a result of this treatment with a corresponding loss in BET surface area from 770 to 390 m2/g. The incorporation of TPA + into the amorphous siliceous walls of SBA-15 is confirmed by 13C{1H} CP MAS NMR experiments and by TGA. The final objective is to synthesize an aluminosilicate with accessible acid sites on the inner surface of the mesopores.
55 2. M A T E R I A L S A N D M E T H O D S 2.1. Materials SBA-15 was prepared following a protocol adapted from the original work by Zhao et al [2]. 4.0 g of the EO20PO70EO20 triblock copolymer P-123 (BASF) is added to a mixture of 19.08 g of 37 wt. % HC1 and 97.1 g of deionized water at 35 ~ with stirring. After the polymer dissolves, 8.5 g of tetraethyl ortho-silicate (Aldrich) is added and stirred at 35 ~ for 20 h. The mixture is heated at 80 ~ statically for 24 hrs in a Teflon container. The product is filtered and washed w i t h - 3 L of deionized water and dried overnight at room temperature. The materials were calcined by heating in air from room temperature to 300 ~ in 5 hrs, then holding at 300 ~ for 12 hrs.
In a typical preparation, 1 g of calcined SBA-15 was impregnated with a liquid mixture of 0.89 g of glycerol and 0.1 g of aqueous (TPAOH) (40% solution) [2]. This mixture was then heated in a Teflon container at 120 ~ for 10 days under static conditions. The treated material was then washed with 1 L of deionized water and dried overnight at room temperature. The calcined form of the treated material is obtained by heating in air at a rate of 1~ to 500 ~ then holding at 500 ~ for 6 hrs. 2.2. Measurements The PXRD patterns were obtained using a Philips X'pert system with Cu KV radiation (8 = 1.54186 A~). SEM images were recorded using a Hitachi S-4000 field emission microscope. Nitrogen adsorption and desorption isotherms were obtained at 77 K using a Micromeritics ASAP 2010 volumetric adsorption analyzer. Before the measurements, the samples were outgassed overnight at 200 ~ 29Si MAS and 13C-{1H} CP MAS NMR spectra were recorded using a Bruker MSL 300 MHz spectrometer operating at resonance frequencies of 59.627 and 75.468 MHz respectively under conditions of magic-angle spinning at 3 kHz at room temperature; ~/3 pulse lengths of 4 gs were used to acquire one-pulse 29Si spectra employing a 90 s relaxation time between each scan. The 29Si MAS spectra and the 13C-{1H} CP MAS NMR spectra were referenced to 2, 2-dimethyl-2-silapentane-5 sulfonate (DSS) and hexamethylene benzene (HMB) respectively. TGA were performed using a Cahn TG-121 microbalance with a heating rate of 5 ~ from room temperature to 800 ~ in air. Transmission electron micrographs were taken on a JEOL 2010F field-emission electron microscope operating at 200 kV. The samples for TEM were prepared by dispersing a large number of particles of the materials through a slurry in acetone onto a lacey carbon film on a Cu grid. 2.3. Methods The BET specific surface area was calculated in the relative pressure range between 0.06 and 0.2. The single point total pore volume was determined from the amount desorbed at a relative pressure of 0.95. The pore size distribution curve came from the analysis of the desorption branch of the isotherm. The pore size distributions were determined using the Halsey equation for multilayer thickness and the calculation procedure proposed by Barrett, Joyner and Halenda (BJH) [9]. The wall thicknesses were calculated as wt = ao- DBm (ao = average hexagonal unit cell dimension and DBJH = pore diameter). The inner surface area of the primary mesopores (Sp) was geometrically calculated by assuming that the pores are perfect cylinders with diameter = DBJH.
56 3. RESULTS AND DISCUSSION A new protocol has been developed for the incorporation of TPA + into SBA-15 with subsequent calcination to form a novel porous material. Starting with the calcined form of SBA-15 as a mesoporous precursor, we aim to transforming the thick amorphous pore walls into domains of silicalite-l-like structures using TPA + as the organic SDA. For this treatment TPAOH was used to provide the TPA + ions and also act as a base. Glycerol (and some water) were used as solvents, also helping in the recrsytallization of the silica phase. The PXRD patterns at low angles indicate that the original hexagonal mesoporous structure of SBA-15 (as indicated by the dl00, dll0 and d200 peaks) is retained with a slight decrease in the unit cell dimension from 107 to 105 A (Figure 2). SBA-15 ...... TPA-SBA- 15 calcined
r.~
k_
0
~
0.5
1
7
1.5
.
2 2.5 2 theta (degrees)
...... : ........ ~.-=-::7...2 ............ ~. . . . .
3
3.5
.-22.. . . . . . . . . . . ;
4
Figure 2. PXRD patterns of SBA' 15 and TPA+-SBA - 15 calcined. As desired, the wide-angle PXRD patterns for the material do not have the characteristic peaks of silicalite-1. This result is as expected because the domains of silicalite-l-like structures formed are probably too small to give rise to measurable PXRD peaks [10]. As the wall thickness of SBA-15 is - 59 A the organized silica structures formed within its pore walls can only be comparable in size to a few unit cells of ZSM-5. PXRD patterns of ZSM-5 crystals consisting of different number of unit cells were calculated using the Cerius 2.0 simulation software (Figure 3). The broad peaks appearing as a result of either one, two, three unit cell cubes or a sum of the above cannot be detected when present in a largely amorphous silica environment of SBA-15. Hence this direct evidence for the formation of silicalite-1 structures cannot be obtained.
57
Figure 3. Calculated PXRD patterns of ZSM-5 crystals consisting of different number of unit cells. SEM images indicate that at the micron level the particle morphology is unaffected by the treatment but at the submicron level the surface of the particles is modified. Although the objective was to transform the structure of the silica phase primarily at the inner surface of the mesopores, the external surface of the SBA-15 particles is readily accessible to the TPA + molecules and the subsequent reaction is unavoidable. TEM images of the sample before and after treatment indicate that the hexagonal mesoporous structure is indeed retained with a significant increase in average pore diameter (Figure 4).
(a)
(b)
Figure 4. TEM images (a) perpendicular and (b) through the pores of TPA+-SBA - 15 calcined. Nitrogen adsorption and desorption experiments show that although the total pore volume (Vt) remains the same the pore structure is significantly modified with a-~20 A increase in the approximate pore diameter (Figure 5). This information along with the unit cell size dimensions was used to show that the wall thickness decreases b y - 2 2 A. The BET surface area (SBET) decreases b y - 5 0 %. This loss in surface area corresponds to the contribution to the total surface area by the fine microporous channels existing in the original SBA-15 material [11-12]. From sorption experiments on similar treated samples at the intermediate
58 stage containing the organic SDA (TPA+-SBA-15), it is shown that there is a definite increase in porosity on removal of the organic, which can be attributed to the additional micropores formed by the TPA + molecules. .,z
500
O
o
~SBA-15
~SBA-15
400
-"TpA-s~A-~,ca,c./ / :....."
r./3
o
6
-" T P A - S B A - 1 5
calc.
300
<@
o ~~ 2 0 0
~
O
O
o
>
~ &2 o
100 I
0 0
I
I
I
0.2 0.4 0.6 0.8 1 Relative Pressure (P/Po)
0 0
50 100 150 Pore Diameter (A)
200
Figure 5. Nitrogen sorption isotherms and pore size distributions of SBA-15 and TPA+-SBA 15 calcined. The d~00 spacings and the unit cell dimensions obtained via PXRD and the sorption data including the average pore diameters, BET total surface areas, inner surface areas due to the primary mesopores and total pore volumes alongwith the wall thickenesses are summarized in Table 1. Table 1.
~X~and_s0~tion~c~har~acter!stics,ofthemater!~a! at yarious~stag~es:................................................................................................................ Sample . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
SBA-15 TPA-SBA-15 calc.
dl00 a0 DBJI~ wt SBzT Sp Vt (~) .........................(~) .........................(~) .............................. .(~)...............(m2g-.1)......(m2 g~!)............(cm3._g~!) .... 90.9 107 48 59 770 520 . 0.73 89.2 105 68 37 390 380 0.73
29Si MAS NMR spectra show a significant loss of Q2 and Q3 surface species as a result of the treatment (Figure 6 (a), (b) and (c)). Quantitative information regarding the Q2, Q3 and Q4 species in the original SBA-15 and in the treated materials is summarized in Table 2. This information along with the sorption results suggests that the pore walls of SBA-15 are condensed and densified by the treatment. TGA of the TPA-SBA-15 samples reveal a 3-4 % weight loss event at an intermediate temperature of 300 ~ which can be attributed to the presence of TPA + incorporated into the mesoporous framework. 13C-{~H} CP MAS NMR spectra of the TPA+-SBA-15 samples further confirm this (Figure 6 (d), (e) and (f)). Apart from the presence of glycerol, these spectra show that the TPA + molecules are present in a silicalite-l-like environment indicated by the two peaks at 16.31 and 11.43 ppm.
59 Q4
Q3 Peaks of TPA +
(a)
(d)
Q2
(b)
j
~
~
(e)
Glycerol
(f)
(c)
-80
-120 (ppm)
-160
88 66 44 22 (ppm)
0
Figure 6. 298i MAS NMR spectra of (a) SBA- 15, (b) TPA+-SBA - 15 and (c) TPA+-SBA - 15 calcined and 13C-{1H} CP MAS NMR spectra of TPA+-SBA-15 (d) deconvoluted (e) simulated and (f) experimental. Table 2.29Si MAS NMR characteristics of the material at various stages. Sample _ (%) ........................................................... SBA-15 4 TPA+-SBA - 15 TPA+-SBA - 15 calcined -
(%) .................................................... (0/0_).... 32 64 11 89 > 90
In this study, TPA + was chosen as the organic SDA to form organized silica structures similar to the model zeolite silicalite-1. This treatment has since been extended to the use of other SDA's such as tetramethyladamantammonium to "imprint" the more complicated cuplike structures of the zeolite MCM-22 on the inner surface of SBA-15. In conclusion, we have successfully developed a protocol for the incorporation of the organic SDA, TPA +, for the zeolite silicalite-1, into the mesoporous material SBA-15. As a result of this treatment the framework mesoporous structure of the material is retained with an increase of 20 A in the average pore diameter. The silica phase is further condensed and densified with a decrease of 22 A in the wall thickness. The incorporation of TPA + is confirmed by ~3C-{1H} CP MAS NMR experiments and thermogravimetric analyses. The domains of silicalite-1 formed are too small to be detected by XRD. In order to detect the formation of silicalite-l-like structures catalytic tests must be performed on aluminum
60 containing samples. Similar initial results have been obtained for A1-SBA-15 as for the allsilica materials 4. ACKNOWLEDGMENTS We would like to acknowledge BASF for providing the P-123, Dr C. Ni for the TEM images and NSF for funding this research (NSF Career Award CTS-9733066). REFERENCES
1.
C.T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710; J. S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T. -W. Chu, D. H. Olson, E. W. Sheppard, S. B. McCullenm, J. B. Higgins and J. L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. 2. D. Zhao, Q. Huo, J. Feng, B. F. Chmelka and G. D. Stucky, J. Am. Chem. Soc., 120 (1998) 6024. 3. J.Y. Ying, C. P. Mehnert and M. S. Wong, Angew. Chem. Int. Ed., 38 (1999) 56. 4. K.R. Kloetstra, H. van Bekkum and J. C. Jansen, Chem. Commun., (1997) 2281. 5. B.T. Holland, L. Abrams and A.Stein, J. Am. Chem. Soc., 121 (1999) 4308. 6. L. Huang, W. Guo, P. Deng, Z. Xue and Q. Li, J. Phys. Chem. B, 104 (2000) 2817. 7. Y.J. Wang, Y. Tang, Z. Ni, W. M. Hua, W. L. Yang, X. D. Wang, W. C. Tao and Z. Gao, Chem. Lett., (2000) 510. 8. D. Margolese, J. A. Melero, S. C. Christiansen, B. F. Chmelka and G. D. Stucky, Chem. Mater., 12 (2000) 2448. 9. E.P. Barrett, L. G. Joyner and P. P. Halenda, J. Am. Chem. Soc., 73 (1951) 373. 10. J. L. Schlenker and B. K. Peterson, J. Appl. Cryst., 29 (1996) 178. 11. M. Kruk, M. Jaroniec, C. H. Ko, R. Ryoo, Chem. Mater., 12 (2000) 1961. 12. S. Jun, S. H. Joo, R. Ryoo, M. Kruk, M. Jaroniec, Z. Liu, T. Ohsuna, O. Terasaki, J. Am. Chem. Soc., 122 (2000) 10712.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rightsreserved.
61
Synthesis and characterization o f p o l y m e r - t e m p l a t e d o r d e r e d silica with cage-like m e s o s t r u c t u r e Jivaldo R. Matos, a Michal Kruk, Lucildes P. Mercuri a and Mietek Jaroniec Department of Chemistry, Kent State University, Kent, Ohio 44242, USA
Advances recently made in our research group in the synthesis and characterization of ordered silicas with large cage-like mesopores are overviewed with a focus on materials templated using a B50-6600 poly(ethylene oxide)-poly(butylene oxide)-poly(ethylene oxide) (EO39BO47EO39) triblock copolymer, as proposed by Yu et al. The mesopore diameter of these silicas can be controlled by changing the initial synthesis temperature and by applying an additional higher-temperature treatment, but the excessively long treatment time may lead to a loss of the pore entrance size uniformity. Not only tetraethyl orthosilicate (TEOS), but also a cost-effective sodium silicate can be used to assemble these large-pore silicas, but TEOS provides more flexibility in terms of the structure tailoring. All the obtained silicas exhibited appreciable microporosity, as expected from the fact that they were templated by a polymer with EOn blocks. The pore entrance size in selected samples was determined by monitoring changes in gas adsorption properties after the surface modification with judiciously chosen organosilanes and it was shown that the pore openings can be made uniform in diameter and either primarily in the micropore or in the mesopore range depending on the synthesis temperature. There is also evidence that the surface-modificed silicas with cage-like mesopores may exhibit molecular sieving effects, because the pore entrance size within subnanometer range can be attained.
1. INTRODUCTION The last eight years brought the discovery of ordered silicas and organosilicas with cagelike mesopores [1-3] and a remarkable progress in their synthesis, characterization and application [4-40]. These materials can be synthesized using both cationic surfactants [116,35-37] and non-ionic oligomer or block-copolymer templates [17-29], many of which are commercially available. The pore (cage) diameter attainable for silica structures spans from the lower end of the mesopore range [4] to about 12 nm [27-29,40], and the materials can be prepared in the form of powders, thin films [10-12,14-16,19], and fibers [18]. Ordered silicas with cage-like mesopore structures (OSCMSs) have already been successfully frameworkmodified in order to incorporate heteroatoms of catalytic properties [30-32]. OSCMSs were also used to grow well-aligned carbon nanotubes [33] and to template the formation of 3Permanent address: Instituto de Quimica da Universidade de Sao Paulo. C.P. 26.077, 05599970, Sao Paulo, SP, Brazil.
a
62 dimensionally (3-D) ordered carbon frameworks stable upon template removal [34]. However, some important aspects of the synthesis and characterization of OSCMSs have been addressed only recently. First, the structural types of many of these materials were tentatively assigned on the basis of X-ray diffraction (XRD) and transmission electron microscopy (TEM) [1,2,17], but require verification and confirmation. In addition, details of their pore structure, and connectivity as well as framework properties, require proper elucidation. This is prompted by findings that one of OSCMSs (SBA-2) is not a pure phase and that the pores in these materials are 2-dimensionally connected, although the porous structure itself is 3-dimensional [8], and that some ordered block copolymer-templated silicas exhibit microporosity in their pore walls [41]. Recently, some of the OSCMS structures, including SBA-1, SBA-6 and SBA-16, have been solved using the electron crystallography [38], and their original structural assignments [1,17] were confirmed, but solutions of other structures are yet to be published and may differ from the structures originally suggested. For the first time, the electron crystallography provided detailed information about the connectivity of mesopores in the OSCMS structures, including the size of pore entrances, which were found to be much smaller than the pore (cage) diameters. Second, methods suitable for reliable determination of the pore diameter and the pore entrance size need to be identified or developed. The aforementioned electron crystallography method is a major step in this direction, but this approach is only tractable for highly ordered materials with appreciable sizes of ordered domains. A more practical method, but restricted only to the determination of pore diameter, was developed for spherical pores based on nonlocal density functional theory (NL DFT) of gas adsorption data [40]. This work provided strong indications that the pore diameters of OSCMSs are substantially larger than those estimated using standard adsorption methods [42], and somewhat larger than those assessed using a method [43] calibrated for cylindrical rather than spherical pores. The presence of intrawall pores in many OSCMSs, both templated by alkylammonium surfactants and oligomers/polymers, was also suggested. Third, convenient approaches for the synthesis of OSCMSs with tailored pore size and cage opening size need to be identified. The standard method is to use surfactants of different sizes [4,9,38], but there were also indications that in the case of polymer-templated syntheses, the temperature control allows one to tailor the pore diameter [26]. Forth, cost-effective syntheses of OSCMSs need to be developed. The use of oligomers and polymers as templates is a major step toward this goal, but another is to substitute the expensive tetraethyl orthosilicate (TEOS) by a cheaper silica source, such as sodium silicate. This has recently been accomplished for oligomer-templated OSCMSs, but the possibility to assemble OSCMSs using block copolymers, which would potentially lead to large-pore materials, was only mentioned [20]. Our recent studies provided important contributions to the aforementioned four issues in the OSCMS synthesis and characterization. This includes (i) the evidence that a triblockcopolymer-templated OSCMS has a strongly microporous framework [29], (ii) the development of a simple and practical method for determination of the pore entrance size in OSCMSs [39], (iii) the finding that not only the pore diameter, but also the pore entrance size can be controlled by changing the synthesis temperature in block copolymer-templated syntheses [39], and (iv) the elaboration of the synthesis of large-pore OSCMS using a costeffective sodium silicate [29]. These developments are discussed hereafter.
63
2. E X P E R I M E N T A L
FDU-1 silicas were synthesized as proposed by Yu et al. [27,28]. The synthesis mixture composition was 1 TEOS : 0.00735 B50-6600 : 6 HC1 : 155 H20, where B50-6600 is a poly(ethylene oxide)-poly(butylene oxide)-poly(ethylene oxide) triblock copolymer (EO39BOa7EO39).The initial synthesis step was performed at room temperature, 313 K or 333 K. In some cases, an additional period of heating at 373 K was employed. A typical synthesis was as follows [29]. 1.83 g ofB50-6600 was dissolved in 110 g of 2 M HC1 by stirring for 12 hours at room temperature, and a homogeneous mixture was obtained. Subsequently, 7.61 g (8.t6 mL) of TEOS was added and the stirring was continued for another 24 h at room temperature, during which precipitation took place. The precipitate was filtered, washed with water, dried at room temperature, and calcined under nitrogen, which was then switched to air at 813 K. Alternatively, sodium silicate (Aldrich; 14% NaOH, 27% SiO2, and 59% H20) was used as a silica source instead of TEOS. In this case, the synthesis mixture composition was 1 SiO2 : 0.778 NaOH : 0.00735 B50-6600:6 HC1 : 162 H20, and the polymer mixture in HC1 solution was cooled down to 288 K before the addition of the silica source. Nitrogen adsorption isotherms were measured on a Micromeritics ASAP 2010 volumetric adsorption analyzer. Before these measurements, samples were degassed under vacuum for at least 2 hours at 473 K. Weight change curves were recorded under nitrogen atmosphere on a TA Instruments TGA 2950 thermogravimetric analyzer using a high-resolution mode with a maximum heating rate of 5 K min -1. The BET specific surface area [42] was evaluated from data in the relative pressure range from 0.04 to 0.2. The total pore volume [42] was estimated from the amount adsorbed at a relative pressure of 0.99. The external surface area and the sum of the primary mesopore volume and micropore volume were evaluated using the cts plot method [42,44] in the C~s plot range from 1.75 to 2.2. The micropore volume and the sum of the primary mesopore surface area and external surface area were determined in the ~s range from 0.9 to 1.2. The standard reduced adsorption ~Xs is defined as the amount adsorbed at a given relative pressure divided by the amount adsorbed at a relative pressure of 0.4 for the reference adsorbent. Macroporous silica LiChrospher Si-1000 was used as a reference adsorbent [44]. The pore size distribution (PSD) was calculated using the Kruk-JaroniecSayari (KJS) method [43], which was calibrated for cylindrical pores and consequently, the pore diameters obtained for cage-like pores of FDU-1 are expected to be somewhat underestimated [29,40]. The statistical film thickness curve suitable for calculation of PSD was reported elsewhere [44]. The pore diameter is defined as a maximum o f K J S PSD.
3. R E S U L T S AND D I S C U S S I O N Yu et al. recently reported that OSCMS (referred to as FDU-1) with a structure identified as cubic Im3m can be synthesized in a wide range of conditions using B50-6600 poly(ethylene oxide)-poly(butylene oxide)-poly(ethylene oxide) triblock copolymer template [27,28]. These authors reported that the pore diameter of FDU-1 is 12 nm, but did not discuss whether it is possible to tailor it, and did not elucidate the pore entrance size. The cage-like nature of pores of FDU-1 was clear from the shape of the adsorption-desorption hysteresis loop on the nitrogen adsorption isotherm [28], because the hysteresis loop was broad, featured sharp capillary condensation and evaporation steps, and the latter step was located at a relative pressure corresponding to a lower limit of adsorption-desorption hysteresis (0.4-
64 0.5). We have synthesized a series of samples using the same synthesis mixture composition and similar synthesis conditions as those employed by Yu et al. We used one-step and twostep procedures (the latter with an additional higher-temperature treatment) and varied the synthesis temperature and time. Yu et al. reported that FDU-1 forms at temperatures up to 333 K and indeed silicas with adsorption properties similar to those reported for FDU-1 were obtained when the initial synthesis temperature was between room temperature and 333 K [29]. The pore diameter of these silicas was increased from 8.7 to 9.5 nm by increasing the temperature of the initial step from room temperature to 313 K. Further pore diameter enlargement to 11.2 nm was achieved when this step is followed by heating at higher temperature (for instance 373 K). However, in this case, an excessively long treatment led to the loss of uniformity of the pore entrance size, as seen from the fact that desorption from the pores started to take place well below the lower limit of adsorption-desorption hysteresis (relative pressure of 0.4-0.5; see data for samples A and C in Figure 1), suggesting the development of entrances of diameter above 5 nm, unlike in the case of good-quality FDU-1 (see data for sample B and [27-29]). When the first step of the synthesis was carried out at room temperature, the structural degradation was not observed after 12, or sometimes even 24 hours of heating at 373 K (see data for sample B), but was evident for longer heating times (see data for samples A and C). It was already reported that the increase in the synthesis temperature allows one to enlarge the pore size of polymer-templated ordered mesoporous silicas with 2-D hexagonal structure [ 17]. However, the indication that this behavior extends over polymer-templated OSCMSs was briefly reported just recently [26] for SBA-16 silica [ 17]. Our study provided additional evidence for the viability of this method of the pore size control for polymer-templated OSCMSs (see PSDs for samples D-F in Figure 2). 6oo
|
|
i
,
r
[--.
500
o
~0 400
A
9
[--,
B
i
i
o
D
9
E
300
400 300 o
or ~
<
i
"7
"7 exl)
200
200
<
+.a
100 < 0.0
!
i
1
i
0.2
0.4
0.6
0.8
Relative Pressure
0
1.0
U
0.0
1
i
i
!
0.2
0.4
0.6
0.8
1.0
Relative Pressure
Figure 1. Nitrogen adsorption isotherms for samples synthesized using B50-6600 as a template and TEOS (A-C) or sodium silicate (D-E) as a silica source. Samples A-D were synthesized at room temperature and subsequently heated (A-C only) for 1 day (A,B) or 4 days (C). Samples E and F were synthesized at 318 K, which in the case of sample F was followed by heating at 373 K for 6 hours (data for samples A and D-F taken from Ref. 29). It was reported that SBA-15 silica templated by poly(ethylene oxide)-poly(propylene oxide)-poly(ethylene oxide) triblock copolymer exhibited some microporosity [45], although
65 its origin was not identified. We have confirmed the occurrence of microporosity in SBA-15, and explained its formation as an effect of penetration of EOn blocks of the template in the silica pore walls [41 ]. On the basis of this explanation, we suggested [41 ] that the occurrence of microporosity in the pore walls is a general behavior that extends over SBA-15 and, most likely, other silicas templated by polymers with EOn blocks. The presence of microporosity in SBA-15 pore walls causes that the large, cylindrical mesopores of this material are connected, rather than isolated as in the case of MCM-41. Consequently, it was possible to synthesize 3D ordered platinum and carbon replicas of SBA-15 [34,41]. As expected, FDU-1 silicas were also found to be microporous. This is seen from C~s-plots, whose linear regions that preceded the increase in adsorption related to capillary condensation intercepted the Amount Adsorbed axis significantly above the origin. The corresponding micropore volumes ranged from 0.18 to 0.27 cm 3 g~ for different samples [29]. It can be expected that other OSCMSs templated by oligomers and polymers with EOn blocks also exhibit microporosity in their pore walls. .
.
.•'=fi
.
.
.
350
0.12'
~n' 0.10
.
o *
~ ~
D E
300 250
0.08
200
ff~ ~9 0.06
~
150
0.04
~
100
b~ 0.02
~ <
50
2
o.oo
o
3
6
9
Pore Size (nm)
12
15
0.0
0.4
0.8
1.2
1.6
2.0
2.4
Standard Adsorption c~s
Figure 2. Pore size distributions for samples D-F (see caption to Figure 1) and the C~s-plot for FDU-1 silica synthesized from TEOS at room temperature (G). Data for D-F taken from [29]. The problem of determination of the pore entrance size in OSCMSs is crucial from the point of view of their prospective applications as selective adsorbents, size- or shape-selective catalysts, supports for chemically bonded functional groups, templates, immobilization media, and so forth. The OSCMS pore entrance sizes are too small to be elucidated from the position of desorption branches of gas adsorption isotherms using known concepts in adsorption data analysis [40,47,48]. Moreover, no reports have indicated that the pore opening sizes can be reliably deduced from PSDs, so the OSCMS pore entrance dimensions had been unknown until the electron crystallography method was elaborated [38]. So far, this powerful approach allowed for elucidation of the pore entrance size in several OSCMS samples, including SBA-1, SBA-6 and SBA-16 silicas. However, this method requires a powerful TEM instrumentation, and is suitable for samples that are highly ordered and exhibit an appreciable size of ordered domains. Therefore, it is inapplicable for some important silicas with cage-like pores that are not ordered [48,49], and in any case, it does not appear to be practical for routine characterization of OSCMSs. Recently, we have developed a practical method for determination of the pore entrance size in OSCMSs and related materials with organosilica framework [39]. This novel method is based on the monitoring of changes in
66 pore accessibility brought about by surface modification with a series of organosilanes with a gradually increasing size. In practice, OSCMS is surface-modified with several judiciously chosen organosilanes, and gas adsorption isotherms of the resulting materials are measured. The size of the smallest organosilane whose introduction leads to a complete pore blockage (which manifests itself in the reduction of the adsorption capacity at higher relative pressures by one or more orders of magnitude) is related to the pore entrance size, taking into account the size of gas molecules used for adsorption studies. The application of this novel methodology allowed us to determine that for FDU-1 silica synthesized at room temperature, the pore entrance diameter was above about 1.2 nm, an average diameter was below about 1.4 nm, and there were essentially no entrances of diameter above 1.9 nm. The pore entrance size in FDU-1 synthesized at room temperature and subsequently heated at 373 K for 6 hours was substantially higher, as it was estimated to be above 1.9 nm, but below 2.9 nm with no evidence of any pore entrances of diameter above the latter value. This showed that for the same polymeric template, the OSCMS pore entrance size can be enlarged nearly two-fold simply by applying the higher-temperature treatment. It is important to note that for FDU-1 synthesized at room temperature, we observed that an increase in the length of alkyl chain of the surface modifier by just one carbon atom transformed a porous structure from wellaccessible to largely inaccessible to gaseous nitrogen [39]. This behavior strongly indicates the pore opening size in the FDU-1 sample considered was uniform and that the aforementioned modified sample with still accessible pores exhibited the entrance sizes in a subnanometer range. Thus, it is expected that the surface-modified FDU-1 that would exhibit molecular size selectivity can be readily synthesized [39]. Our method for the pore entrance size elucidation does not provide some important structural information, such as the shape of the entrance and the average connectivity in the structure, but is applicable for both ordered and disordered silicas [48,49]. In addition, our method allows one to probe the pore entrance dimensions within the entire sample, whereas the electron crystallography probes materials on a local level, allowing one to solve structures even for single particles, but does not provide an averaged information for the whole material, which our method does. So, the two approaches are complementary, especially as the first one can be used for routine analysis, but provides information about the pore entrance size only, whereas the second one provides the solution of the entire structure, but is not practical for the routine analysis. Yu et al. [27,28] originally used TEOS as a silica source for FDU-1 synthesis. We have demonstrated that when this reagent is substituted by a cost-effective sodium silicate [29], silicas with adsorption properties analogous to those of FDU-1 (see Figure 1) and with similar specific surface areas and pore volumes can be synthesized. Thermogravimetric studies of assynthesized samples assembled using TEOS and sodium silicate showed no appreciable differences in the triblock copolymer template content and its decomposition temperature range, additionally suggesting that sodium silicate can be used to assemble the FDU-1 silicas [29]. However, the synthesis from sodium silicate was successful only under more restricted conditions, when compared to the original procedure. In particular, when sodium silicate was used, no structure with uniform mesoporosity was obtained at 333 K, and the application of the additional heating step at 373 K led to the structural degradation after very short periods of time. For instance, a sample synthesized at room temperature and subsequently heated at 373 K for 6 hours already showed signs of structural degradation [29]. We found that the synthesis of FDU-1 from TEOS provides more flexibility in terms of the pore diameter tailoring, as the latter can be adjusted by 2.5 nm (from 8.7 to 11.2 nm) by varying the synthesis temperature in one-step and two-step procedures, whereas the range of pore diameters attainable using sodium silicate was restricted to within 1.8 nm (8.5-10.3 nm) [29].
67 4. CONCLUSIONS When B50-6600 template is used, ordered silicas with large cage-like pores can be synthesized using not only TEOS, but also a cost-efficient sodium silicate. The pore diameter of these materials can be controlled by choosing an appropriate initial synthesis temperature and employing an additional higher-temperature treatment. The pore entrance diameter can also be controlled in a similar manner and is primarily in either the micropore or mesopore range depending on the synthesis conditions. The pore entrance size of one of the FDU-1 silicas discussed herein was shown to be decreased to the subnanometer range by employing a simple surface modification procedure, which allows one to obtain a new kind of a mesoporous zeolite analogue. Extended high-temperature treatments led to the loss of uniformity in the pore opening size, which manifests itself in the formation of pore openings of diameter above about 5 nm. FDU-1 exhibits a high amount of micropores in the mesopore walls, which appears to result from the inherent tendency of EOn blocks to be occluded in silicate pore walls during formation of ordered silicas.
5. A C K N O W L E D G M E N T S M. J. acknowledges support by NSF Grant CHE-0093707. J. R. M. and L. P. M. thank for support Fundacao de Amparo a Pesquisa do Estado de Sao Paulo (FAPESP, Brazil), fellowships under grants 99/11170-5 and 99/11171-1. The authors also thank Dr. Rene Geiger from the Dow Chemical Company for providing B50-6600 triblock copolymer.
REFERENCES
1. Q. Huo, D. I. Margolese, U. Ciesla, P. Feng, T. E. Gier, P. Sieger, R. Leon, P. M. Petroff, F. Schuth and G. D. Stucky, Nature, 368 (1994) 317. 2. Q. Huo, R. Leon, P. M. Petroff and G. D. Stucky, Science, 268 (1995) 1324. 3. S. Inagaki, S. Guan, Y. Fukushima, T. Ohsuna and O. Terasaki, J. Am. Chem. Soc. 121 (1999) 9611. 4. M.J. Kim and R. Ryoo, Chem. Mater., 11 (1999) 487. 5. S. Che, Y. Sakamoto, O. Terasaki and T. Tatsumi, Chem. Mater. 13 (2001) 2237. 6. S. Che, S. Kamiya, O. Terasaki and T. Tatsumi, J. Am. Chem. Sot., 123 (2001) 12089. 7. V. Goletto, V. Dagry and F. Babonneau, Mat. Res. Soc. Symp. Proc., 576 (1999) 229. 8. W. Zhou, H. M. A. Hunter, P. A. Wright, Q. Ge and J. M. Thomas, J. Phys. Chem. B, 102 (1998) 6935. 9. H.M.A. Hunter and P. A. Wright, Microporous Mesoporous Mater., 43 (2001) 361. 10. S. H. Tolbert, T. E. Schaffer, J. Feng, P. K. Hansma and G. D. Stucky, Chem. Mater., 9 (1997) 1962. 11. Y. Lu, R. Ganguli, C. A. Drewien, M. T. Anderson, C. J. Brinker, W. Gong, Y. Guo, H. Soyez, B. Dunn, M. H. Huang and J. I. Zink, Nature, 389 (1997) 364. 12. D. Zhao, P. Yang, D. I. Margolese, B. F. Chmelka and G. D. Stucky, Chem. Commun., (1998) 2499. 13. Y. Lu, H. Fan, A. Stump, T. L. Ward, T. Rieker and C. J. Brinker, Nature, 398 (1999) 223. 14. M. Ogawa and N. Masukawa, Microporous Mesoporous Mater., 38 (2000) 35.
68 15. S. Besson, T. Gacoin, C. Jacquiod, C. Ricolleau, D. Babonneau and J.-P. Boilot, J. Mater. Chem., 10 (2000) 1331. 16. D. Grosso, A. R. Balkenende, P. A. Albouy, M. Lavergne, L. Mazerolles and F. Babonneau, J. Mater. Chem., 10 (2000) 2085. 17. D. Zhao, Q. Huo, J. Feng, B. F. Chmelka and G. D. Stucky, J. Am. Chem. Soc. 120 (1998) 6024. 18. P. Yang, D. Zhao, B. F. Chmelka and G. D. Stucky, Chem. Mater., 10 (1998) 2033. 19. D. Zhao, P. Yang, N. Melosh, J. Feng, B. F. Chmelka and G. D. Stucky, Adv. Mater., 10 (1998) 1380. 20. J. M. Kim and G. D. Stucky, Chem. Commun., (2000) 1159. 21. P. Kipkemboi, A. Fogden, V. Alfredsson and K. Flodstrom, Langmuir, 17 (2001) 5398. 22. C. Yu, B. Tian, J. Fan, G. D. Stucky and D. Zhao, Chem. Commun., (2001) 2726. 23. S. A. E1-Safty and J. Evans, J. Mater. Chem., 12 (2002) 117. 24. C. E. Tattershall, N. P. Jerome and P. M. Budd, J. Mater. Chem., 11 (2001) 2979. 25. W. Zhang, B. Glomski, T. R. Pauly and T. J. Pinnavaia, Chem. Commun., (1999) 1803. 26. C.-P. Kao, H.-P. Lin, M.-C. Chao, H.-S. Sheu and C.-Y. Mou, Stud. Surf. Sci. Catal., 135 (2001). 27. C. Yu, Y. Yu and D. Zhao, Chem. Commun., (2000) 575. 28. C. Yu, Y. Yu, L. Miao and D. Zhao, Microporous Mesoporous Mater., 44-45 (2001) 65. 29. J. R. Matos, L. P. Mercuri, M. Kruk and M. Jaroniec, Langmuir 18 (2002) 884. 30. M. S. Morey, A. Davidson and G. D. Stucky, J. Porous Mater., 5 (1998) 195. 31. L.-X. Dai, Y.-H. Teng, K. Tabata, E. Suzuki and T. Tatsumi, Chem. Lett., (20.00) 794. 32. L.-X. Dai, K. Tabata, E. Suzuki and T. Tatsumi, Chem. Mater., 13 (2001) 208. 33. G. Zheng, H. Zhu, Q. Luo, Y. Zhou and D. Zhao, Chem. Mater., 13 (2001) 2240. 34. R. Ryoo, S. H. Joo, M. Kruk and M. Jaroniec, Adv. Mater., 13 (2001) 677. 35. S. Guan, S. Inagaki, T. Ohsuna and O. Terasaki, J. Am. Chem. Soc. 122 (2000) 5660. 36. Y. Lu, H. Fan, N. Doke, D. A. Loy, R. A. Assink, D. A. LaVan, and C. J. Brinker, J. Am. Chem. Soc. 122 (2000) 5258. 37. A. Sayari, S. Hamoudi, Y. Yang, I. L. Moudrakovski and J. R. Ripmeester, Chem. Mater. 12 (2000) 3857. 38. Y. Sakamoto, M. Kaneda, O. Terasaki, D. Y. Zhao, J. M. Kim, G. Stucky, H. J. Shin and R. Ryoo, Nature, 408 (2000) 449. 39. M. Kruk, V. Antochshuk, J. R. Matos, L. P. Mercuri and M. Jaroniec, J. Am. Chem. Soc. 124 (2002) 768. 40. P. I. Ravikovitch and A. V. Neimark, Langmuir, published on Web 1/23/2002. 41. R. Ryoo, C. H. Ko, M. Kruk, V. Antochshuk and M. Jaroniec, J. Phys. Chem. B, 104 (2000) 11465. 42. S. J. Gregg and K. S. W. Sing, Adsorption, Surface Area and Porosity, Academic Press, London, 1982. 43. M. Kruk, M. Jaroniec and A. Sayari, Langmuir, 13 (1997) 6267. 44. M. Jaroniec, M. Kruk and J. P. Olivier, Langmuir, 15 (1999) 5410. 45. W. W. Lukens, Jr., P. Schmidt-Winkel, D. Zhao, J. Feng and G. D. Stucky, Langmuir, 15 (1999) 5403. 46. J.-S. Lee, S. H. Joo and R. Ryoo, J. Am. Chem. Soc., 124 (2002) 1156. 47. M. Kruk and M. Jaroniec, Chem. Mater. 13 (2001) 3169. 48. W. W. Lukens, Jr., P. Yang and G. D. Stucky, Chem. Mater., 13 (2001) 28. 49. B. Smarsly, C. Goltner, M. Antonietti, W. Ruland and E. Hoinkis, J. Phys. Chem. B, 105 (2001) 831.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 Elsevier Science B.V. All rights reserved.
69
The m o d e l i n g o f wall structure o f siliceous M C M - 4 1 b a s e d on the formation process Yasunori Oumi, a Kazuhiko Azuma, a Takuji Ikeda, b Shintaro Sasaki, a and Tsuneji Sano a School of Materials Science, Japan Advanced Institute of Science and Technology, Tatsunokuchi, Ishikawa 923-1292, Japan; E-mail:
[email protected]
a
b Advanced Materials Laboratory, National Institute for Materials Science, 1-1 Namiki, Tsukuba, Ibaraki 305-003, Japan
The Monte Carlo and molecular dynamics methods in combination with a continuous electron density representation were applied to the framework modeling of siliceous MCM-41. The X-ray diffraction intensities calculated using a computer simulation technique were strongly influenced by an atomic disordering in the wall structure. Namely, the layer structure in the wall was shown to be fitted better than the amorphous structure. It was also found from the electron density maps that the wall structure of MCM-41 is not uniform, namely a large difference in the charge density exists. This indicates that an understanding of the formation process of MCM-41 is needed for the modeling:
I. INTRODUCTION Mesoporous materials such as MCM-41, MCM-48 and SBA-15 have attracted much attention due to their high surface areas and well-ordered large pore systems [1-4]. Consequently, there are a large number of papers concerning the geometrical structural properties. Although X-ray diffraction(XRD), transmission electron microscopy and adsorption analysis are used for getting the reliable information of the mesoporous structure, a satisfactory structural model of the mesoporous materials is still not constructed. However, only few reports concerning the wall structures of the mesoporous materials have been reported [5, 6], because the atomic array in the wall is considered to be short-range ordering. In order to expand further the high performance applications of the mesoporous materials such as hosts, adsorbents or catalysts, an understanding of the surface property and structure of pore wall as well as the geometrical structure must be needed. Recently, computer simulation techniques such as the molecular dynamics and Monte Carlo methods are employed for modeling of MCM-41 [7-12]. Solovyov et al. proposed the heterogenated surface of the pore wall of MCM-41 using the Rietveld method in combination with a continuous electron density representation [ 13-14]. From such a viewpoint, we have tried to characterize the wall structure of MCM-41 by a new model based on its formation process, and report the preliminary result of MCM-41 modeling in this paper.
70 2. SYNTHESIS OF MCM-41 AND SIMULATION 2.1. Synthesis of MCM-41 Siliceous MCM-41 was prepared following the procedure described in the literature [ 15]. The starting synthesis gel was prepared using colloidal silica, cetyltrimethylammonium bromide (CTAB), sodium hydroxide, aqueous ammonia and water. This synthesis gel with molar composition 6 SiO2 9CTAB 91.5 Na20 90.15 (NH4)20:250 H20 was hydrothermally treated at 97 ~ for 4 days. The synthesis pH was threefold adjusted at 10.2 using dilute acetic acid from time to time. The MCM-41 prepared was calcined at 773 K for 20 h to decompose the surfactant. 2.2. Measurements The synchrotron XRD measurements were carried out at room temperature on a highresolution powder diffractometer at BL 15XU SPring-8 [ 16]. The goniometer equipped long Sollar slit of 1~ aperture to decrease axial divergence. The powder was mounted into a rotating 0.3 mm diameter capillary. Conditions of an measurement were as follows: ~. = 1.549604(3) A calibrated by NIST Si powder, scan range of 0.2 ~ < 20 < 10~ step width: 0.01 ~ counting time per step: 1 s. 29Si MAS NMR spectra were acquired using a Varian VXP-400 spectrometer and zirconia rotors at 79.4 MHz with 2000 pulses and 30s recycle delays. Chemical shifts are given as ppm from external tetramethyl silane. Textural properties were determined at-196 ~ using nitrogen adsorption in a conventional volumetric technique by a Belsorp 28SA spectrometer. 2.3. Simulation method The modeling of MCM-41 was conducted in Monte Carlo (MC) and molecular dynamics (MD) methods. The MC calculations were performed using sorption module in the Cerius2 developed by Molecular Simulation Inc., USA. MC method employs the canonical (NVT) ensemble and the burchart-UNIVERSAL potentials parameter set [17-19] for calculating the interaction between molecules. The all MC calculations performed for 300,000 cycle steps at 20 K. The MD calculations were carried out with the MXDTRICL program developed by Kawamura et al [20]. The Verlet algorithm [21] was used for calculation of the atomic motions, while the Ewald method [22] was applied for the calculation of the electrostatic interactions. Temperature and pressure were controlled by means of scaling the atom velocities and unit cell parameters under three-dimensional periodic boundary conditions. The calculations was performed for 4,000 - 12,000 steps with a time steps of 1.0 • 1015 s at 298.0 K. The two-body central force interatomic potentials, Eq. 1, was used for all MD calculations.
Uu=z, zje2/rjj + fo(b~+bj)exp[(a~+aj-r~j)/(b, +bj)]
(1)
Where Zi is the atomic charge, e is the elementary electronic charge, rij is the interatomic distance, and f0 is a constant. In this equation, the first and second terms refer to Coulomb and repulsive interactions, respectively. The parameters ai and bi represent the size and stiffness of the atoms, respectively, in the repulsive interactions. Table 1 shows the potential parameters employed in this study. The details and effectiveness of the two-body interatomic potential for reproducing the experimentally determined crystal structure of ZSM-5 as well as other conditions of the simulations have been reported elsewhere.
71 Both XRD pattern and 29Si MAS 298i MAS NMR module in Cerius2.
NMR spectra were simulated by the XRD module and
All calculations were performed on Silicon Graphics Indigo2 workstations, while the static visualization was done with the Cerius2 program developed by Molecular Simulation Inc., USA. The dynamic visualization was made, with RYUGA codes developed by Miura [23].
Table 1 Potential parameters of Si and O atoms for MD calculations Atom O Si
Zi -1.2 2.4
ai 1.735 1.012
bi 0.126 0.084
2.4. Calculation of electron density projection Electron density projection was simulated by frg developed by Sasaki. The electron density projection along the c axis is determined by Fourier synthesis in the equatorial plane. Two dimensional structure of the hexagonal system is probably centrosymmetric and has dyad axes (space group :p6mm), where the F(hkO)'s are real and F(hkO) = F(khO). Since the amplitudes(IF01 on a relative scale) are obtained from the intensity data, the projection can be calculated by assigning the phase factor (+ 1 or -1) to them. The electron density projected on the point (x, y) was defined here by the average of the density at (x, y, z) along z axis over a repeat distance c = 10 A (assumed for the standard t~-helix): c
=op(xyz)dz =
F o(hkO)cos{2zc(hx + ky)}
(2)
where V is the unit cell volume.
3. RESULTS AND DISCUSSION 3.1. Modeling of the framework structure of MCM-41 The three kinds of MCM-41 framework models were constructed using MC and MD methods. For the modeling of MCM-41, the dummy atoms arranged in a unit lattice were employed as a micellar rod. The lattice parameters and pore size of the synthesized MCM-41 obtained by XRD and N2 adsorption were used as initial parameters for the modeling. Fig. 1 shows the modeling schemes of MCM-41. The models of (b) and (c) are based on the assumption that the pore wall has a layer structure, whereas the wall structure of the model (a) is amorphous. 400 SiO2 molecules were totally generated in MC calculation. In the case of the model (a), 400 SiO2 molecules were generated simultaneously and uniformly distributed after MC calculation. And the dummy atoms were finally removed. This model was designated as the "random model". In the case of the model (b), three different dummy units with different sizes were constructed for formation of MCM-41 with the layer structure and integrated into the MCM-41 structure, designated as "layer model". The MD calculations were performed to stabilize the MCM-41 structure of the (a) and (b) models. In the case of the model (c), the MCM-41 structure was formed through successive accumulation of dummy models. Before integration, MD calculation of the model unit was performed at each step for stabilization of the model unit. In this way, integration were performed one by one, finally the stabilized MCM-41 model was obtained (phased layer model).
72
(a)
(b)
removal of dummy atoms
MC
removal of MC dummy atoms '~ % ~,~ ~ .* L ~ '
9
.:...~.~
,~".'N-
~~
~
.....
~ 9 --~
..
. . . . 4 ' ~
~..,
integration of several unit
~ . ~ .
........
.
.
9
.
...
:;:, ?-:.:5., -4) ~ { 9~ ,
(c)
MC
(1) ~
removal of dummy atoms
~,--:~e7_%c
....... ~
--), ">!';;z:-.-,. /
'ta~-.-~ *.~
I
..,._..]-atlT...: ........l~."..:
. . . ~ .~.
integration of several unit
"
"
~
t ===============_===,==,=~ ~ . + %<>. .,"
Fig. 1 Modeling ofMCM-41 structure. (a) random model, (b) layer model, (c) phased layer model 3.2. X-ray diffraction pattern of the framework structure of MCM-41 The XRD simulations of the three constructed models were performed. Fig. 2 shows the XRD patterns of the constructed models and the synthesized MCM-41 as a reference. The XRD pattern of the synthesized MCM-41 presented a typical four-peak' pattern with a very strong peak at a low 20(d (100)) and three weaker peaks at a higher 20 (d (110), d (200), d (210)). Layer models exhibited a typical XRD pattern with four peaks. However, the peak broadening of the 100 reflection was observed. As it is considered that the intensity of the 100 reflection is very sensitive to the relative contrast between wall and mesopore densities, the observed broadening is probably due to imperfections in pore arrangement than to a finite particle size. On the other hand, in the case of the random model, intensities of the 110 and 210 peaks were relatively week. From the fact that the experimental XRD was
100
1
(a)
110
200
210
b)
~ 9
_=
I
2
t
I
3
I
I
I
I
I
I
4 5 6 2 0 (degree) Fig. 2 Simulated X-ray diffraction patterns of MCM-41. (a) random model, (b) layer model, (c) phased layer model, (d) experiment
73 fitted better to simulated pattern by both layer models than the random model, it found that the peak intensities are influenced by the atomic location in the wall structure. 3.3. 29Si MAS NMR spectra of MCM-41 In order to obtain information about the chemical state of Si in the MCM-41 wall structure, the 29Si MAS NMR spectra were simulated using the phased layer model. Fig. 3 shows 29Si MAS NMR spectra of the synthesized MCM-41 and the phased layer model. In the 29Si MAS NMR spectrum of the synthesized MCM-41, the broad peak a t - - - - l l 0 ppm, assigned to strongly polymerized Q4 Si species, as well as the weak shoulder peak a t - -100 ppm, assigned to Q3 Si species, was observed. In the simulated 29Si MAS NMR spectrum from the phased layer model, the broad peak centered a t - 1l0 ppm was observed. This suggests that there is no difference in the chemical state of Si between the synthesized MCM-41 and the phase layer model. 3.4.
4
-50
Coordination of Si in the framework of
MCM-41 The radial distribution function between Si and O atoms in the MCM-41 wall structure was investigated in order to clarify the difference in the
- 1O0 ppm
Fig. 3 29Si MAS NMR spectra of MCM-41. (a) experiment, (b) phased layer model
/y--
lO 40
(c)
50/
i
- 150
/
0 o
~2 30 0
r(c)
,.Q
~ 2o . ,...(
~
~10
0 1.5
l
1.6
1.7
1.8
1.9
Distance between Si and O (A)
2.0
0
I
1
2
I
I
4
I
6
Distance between Si and O (A)
Fig. 4 Radial distribution function between Si and O Fig. 5 Coordination number of Si. atoms. (a) random model, (b) phased layer model, (a) random model, (b) phased layer (c) MFI type silicalite model, (c) MFI type silicalite
74 coordination state of Si. As shown in Fig. 4, sharp peaks were observed at 1.68 and 1.71 _Ain the radial distribution function for MFI type silicalite. On the other hand, in the radial distribution functions for the random model and the phased layer model, the broad peak was observed around 1.7/~. The bond distances, l(Si-O), evaluated by both models were longer that than from MFI type silicalite. Fig. 5 shows that the coordination number of O surrounding Si atom calculated from the radial distribution function. The coordination number of Si increased with an increase in the Si-O distance. In the l(Si-O) ranging from 1.65 A to 3.0A, the coordination number of Si in MFI structure was almost constant 4, indicating the coordination state of Si in the MFI structure is tetrahedral, while the coordination number for the random model and the phased layer model was not constant. This strongly suggests that the coordination state of Si in the MCM-41 wall structure is not uniform. 3.5. Electron density image of the framework structure of MCM-41 The electron density images were calculated using the integral intensities of Bragg reflections. Fig. 6 shows the electron density maps for the synthesized MCM-41. It is noted that the electron density is not continues. The electron density at the intersections of wall was lower than that at the other parts. Fig. 7 shows that the electron density images calculated using the random model, the layer model and the phased layer model. The wall electron densities for both layer models were not continuous, whereas the image for the random model was continuous. The wall electron densities for both layer models were qualitatively similar to the simulated one using the synthesized MCM-41. The non uniformity of the wall electron density ofMCM-41 have been reported by Solovyov et al. [13-14].
(a)
(b)
(c)
Fig. 6 The electron density projections for synthesized MCM-41. (a) 2-D, (b) 3-D, (c) mosaic
4. Conclusion From all above results, it was found that the peak intensity of XRD pattem derived from the hexagonal structure of MCM-41 is dependent on the modeling method of the wall structure. It was also found that the wall structure ofMCM-41 is not uniform.
75
(a)
(A)
(B)
(C)
Fig. 7 The electron density projections for (A) random model, (B) layer model and (C) phased layer model. (a) 2-D, (b) 3-D, (c) mosaic
REFERENCES 1. C, T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli, J. S. Beck, Nature, 359 (1992) 710. 2. J.S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T. W. Chu, D. H. Olson, E. W. Sheppard, S. B. McCullen, J. B. Higgins, J. L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. 3. U. Cisela, F. Schtith, Microporous Mesoporous Mater., 27 (1999) 131. 4. A. Corma, Chem. Rev., 97 (1997) 2373. 5. A. Sayari, Stud. Surf. Sci. Catal., 102 (1996) 1. 6. P. Behrens, Angew. Chem. Int. Ed. Engl., 35 (1996) 515. 7. B.P. Feuston, J. B. Higgins, J. Phys. Chem., 98 (1994) 4459. 8. M.W. Maddox, J. P. Oliver and K. E. Gubbins, Langmuir, 13 (1997) 1737. 9. R.D. Oldroyd, J. M. Thomas, G. Snakar, J. Chem. Soc., Chem. Commun., (1997) 2025. 10. S. Schacht, M. Janicke, F. Schtith, Microporous Mesoporous Mater., 22 (1998) 485. 11. C. A. Koh, T. Montanari, R. I. Nooney, S. F. Tahir, R. E. Westacott, Langmuir, 15 (1999) 6043. 12. R. G. Bell, in 9M. M. J. Treacy, B. K. Marcus, M. E. Bisher, J. B. Higgins (Eds.), Proceeding of the 12th IZC, Baltimore, Materials Research Soc., (1999) 839. 13. L. A. Solovyov, S. D. Kirik, A. N. Shmakov, V. N. Romannikov, Microporous Mesoporous Mater., 44-45 (2001) 17. 14. V. B. Fenelonov, A. Yu. Derevyankin, S. D. Kirik, L. A. Solovyov, A. N. Shmakov, J.-L. Bonardet, A. Gedeon, V. N. Romannikov, Microporous Mesoporous Mater,, 44-45 (2001) 33.
76 15. J. M. Kim, L. H. Kwak, S, Jun, R. Ryoo, J. Phys. Chem., 99 (1995) 16742. 16. T. Ikeda, A. Nisawa, M. Okui, N. Yagi, H. Yoshikawa, S. Fukusima, to be submitted. 17. L.A. Castonguay, A.K. Rappe, J. Am. Chem. Sot., 114 (1992) 5832. 18. A.K. Rappe, K.S. Colwell, Inorg. Chem., 32 (1993) 3438. 19. The Zeoliotes and Aluminophosphates force field of Erik de Vos Burehart, Ph.D. Thesis, (1992) 'Studies on Zeolites: Molecular Mechanics, Framework Stability and Crystal Growth', Table I, Chapter XII. 20. K. Kwamura, in 9Moleucular Dynamics Simulations, eds. F. Yonezawa, Springer, (1990) 88. 21. L. Verlet, Phys. Rev., 98 (1967) 159. 22. P. Ewald, Ann. Phys., 64 (1921) 253. 23. R. Miura, H. Yamano, R. Yamauehi, M. Katagiri, M. Kubo, R. Vetrivel, A. Miyamoto, Catal. Today, 23 (1995) 409.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rightsreserved.
77
Pore size adjustment of bimodal mesoporous silica molecular sieves Xiaozhong Wang, ab* Tao
D o u , a Dong
Wu band Bing Zhong b
Institute of Special Chemicals, Taiyuan University of Technology, Taiyuan, 030024 China e-mail" wanuxiaozhonu~.tvut, edu.cn
a
...
,....._..
f
bState Key Laboratory of Coal Conversion, Institute of Coal Chemistry, the Chinese Academy of Sciences, Taiyuan, 030001 China Bimodal mesoporous silica (BMS) molecular sieves were synthesized using quaternary ammonium surfactant at room temperature with lower pH values, and their pore sizes were tailored using a simple method by controlling the size of the structure-directing surfactant or incorporating an auxiliary organic solvent such as 1,3,5-trimethylbenzene (TMB) into the reaction systems, which has been used previously to control the pore sizes of MCM-41 mesoporous materials. It was shown that as the surfactant alkyl chain length or the amount of TMB used was increased, the enlargement of the primary mesopore size of BMS materials was accompanied concurrently by the decrease of its secondary mesopoe size, and the degree of the primary mesopore size enlargement (ca. 1.0nm) is far smaller than that of MCM-41 mesoporous materials prepared under similar synthesis conditions, but in contrast the degree of its secondary mesopore size decrease is more sharp (ca.6.4nm). These results may be in connection with the characteristic framework structure of our BMS materials. When the amount of TMB used exceeded a certain degree, the primary mesopore structure of BMS materials was still present but its secondary mesopore structure got collapsed. INTRODUCTION The synthesis of inorganic frameworks with specified and organized pore networks is of potential importance in catalysis[l], separation technology[2] and biomaterials engineering [3]. Since the first synthesis of mesoporous MCM-41 materials[4.5], there has been intense activity in the design and synthesis of a variety of mesoporous solids with different structural features. Such features as pore size, pore size uniformity, interparticle porosity, and stability (thermal and hydrothermal) of these mesoporous molecular sieves were shown to be controlled by a proper choice of synthesis conditions[4-9]. At present, the surfactanttemplated synthetic procedures have been extended to include a wide range of compositions, and a variety Of conditions have been developed for exploiting the structure-directing functions of surfactant. These solids allow fasten diffusion of large organic molecules than the zeolitic and aluminium phosphate-based microporous sieves. These structural characteristics
78 make them potentially useful as catalysts for fluidized catalytic cracking and for the manufacture of fine chemicals. However, the information feedback from the practical industrial process shows that the catalyst used in the large molecules reaction requires a reasonable distribution of two-grade or multi-grade pores, and therefore over a long period of time direct synthesis of inorganic porous materials with two-grade or multi-grade pore distribution is researched for by zeolite chemists. In earlier investigations, we showed that careful controlling alkalinity affords a novel porous materials with well-defined bimodal mesopore size distribution at ambient conditions [11~.! 1]. The materials contain randomly distributed hexagnoal and stripe-like mesoporous channels with uniform pore size and exhibit very large surface areas and pore volumes. The secondary mesopore structure of BMS materials may be formed via the development of incomplete condensation of SiO2species around the adjacent surfactant micelle. The bimodal mesoporous structure of thus formed should be able to be tailored by applying the similar methods with which were used usually in the pore size adjustment of M41S materials. So far, relatively little work has been reported for the pore size mediation of bimodal mesoporous silica mesostructures and no convincing mechanism for such bimodal mesoporous structure formation has been put forward. Undoubtedly, the ability to control framework bimodal mesoporous distribution can be of great value in designing BMS materials as catalysts, ' adsorbents and sensor materials. Accordingly, in the present work we have examined the effect of the structure-directing surfactant size and the addition of auxiliary organic solvent such as 1,3,5-trimethylbenzene on the pore size characteristic framework cross-linking of BMS molecular sieves. At the same time we give a full account of the trend of pore size adjustment of BMS materials and extend on our hitherto proposed formation mechanism. 2. EXPERIMENTAL SECTION
2.1. Synthesis The synthesis procedure for BMS materials was described elsewhere[10.11]. For the purposes of probing the effect of surfactant alkyl chain length and auxiliary organic solvent such as 1,3,5-trimethylbenzene (TMB) on pore size distribution of BMS materials, these samples were prepared typical using CI4H29N(CH3)3Br(C14) and C16H33N(CH3)3Br(C16) as templates. Tetraethylorthosilicate (TEOS) was used as a source of silica, and the pH values of the reaction mixture was adjusted with aqueous ammonia. In each case the reaction mixtures had the following molar composition: 1.0 SiO2:0.2 CI4H29N(CH3)3Br : 0.09 NH3" H20 : 115H20 1.0 SiO2:0.2 CI6H33N(CH3)3Br : 0.3 NH 3"H20 : (0-0.84) TMB : 115H20 The number of molar of ammonia in each reaction mixture was varied relying on surfactants alkyl chain length. When TMB was used as an auxiliary structure director, it was added to the surfactant solution and stirred for 15min before the addition of TEOS. All of the BMS reaction products were washed repeatedly with distilled water in a centrifuger, dried in air at 353K and finally calcined in air at 2K min"~to 823K for 6 h to remove the template.
79 2.2. Characterization
The powder X-ray diffraction pattems (XRD) were recorded using a D/max-2500 powder diffractometer with Cu-K a radiation (40kV, 100mA),0.02~ size and 1 s step time over the range 1~ 0 <8 ~ N2 adsorption isotherms were measures at -196"(2 using a ASAP2000 analyser. The volume of adsorbed N2 was normalized to standard temperature and pressure. Prior to the experiments, samples were dehydrated at 350 ~ for 12h. The pore-size distribution was calculated using the desorption branches of the N2 adsorption isotherm and the Barrett-Joyner-Halenda (BJH) formula. 3. RESULTS AND DISCUSSION 3.1. Effect of surfactant alkyl chain length We have prepared BMS materials by the similar assembly procedure using quaternary ammonium surfactants with different chain length as structure director at room temperature. Figure 1 provides the representative X-ray powder diffraction patterns for the as-synthesized and calcined BMS derivatives formed using C~4 and C~6as structure directors. Each sample exhibites a single very low angle reflection, which seems to display less ordering in the mesostructure with a large unit-cell size. However, it can not be simple regarded as an average of pore-pore correlation distance due to the particularity of bimodal mesoporous framework structure of BMS materials. As the surfactant alkyl chain length is increased, the interplanar spacing dl0 0 of BMS samples is also of the trend of shifting gradually toward lower 2 0 angle, which is consistent with the synthesis results of MCM-41 mesoporous materials 8000
A
4000
B
= 4000 E 2000
b
b
a
a
0 0
2
4
6
8
0 10
0
O_Theta
2
4
6
8
10
2-Theta
Figure 1. Powder X-ray diffraction pattems of as-synthesized (A) and calcined (B) BMS samples prepared using C~4 (a) and C~6 (b) surfactant as templates prepared in similar conditions. There are no significant changes upon calcinations, except for the expected increase in XRD peak intensity and lattice contraction due to the higher removal of the contrast-matching surfactant. This result is consistent with the retention of the framework bimodal mesoporous structure upon complete removal of the surfactant from the framework.
80
C14
1200 "7
c~o
800
A
t:m e~
400
0
"x3
0
,.Q
o
0
r,c]
1200800 C16
_
~
C16
<
400 i
0
0
i
,
~t
I
0.2 0.4 0.6 0.8
1
Relative Pressure (P/Po)
10
100
1000
10000
Pore Size (/~)
Figure 2. N 2 adsorption isotherms and corresponding pore size distribution curves of BMS samples prepared using C~4 and C~6surfactant as templates Figure 2 shows the N 2 adsorption isotherms and corresponding BJH pore size distribution curves for calcined BMS samples. The samples exhibit type IV isotherms as expected for mesopores but with a characteristic hysteresis loop lifted up sharply in the P/Po region of 0.81.0. This may indicate that a change in the texture has occurred on the mesoporous frameworks of the product and suggest the presence of noticeable amount of secondary mesopores, i.e. filling of the framework-confined mesopores occurred at p/po=0.2-0.4 and p/po=0.8-1.0, respectively. This can be confirmed from BJH plots in Figure 2 (right), and two samples all show a well-confined bimodal mesopore distributions. Table 1 summarizes the effect of template sizes on the structural properties of BMS materials. It is especially Table 1. Structural properties of calcined BMS materials prepared using C~4 and C~6 surfactant. Primary mesopore Secondary mesopore SBET(m2g"l) Vs(cm3g"~) Ds(nm) Sample dl00(nm) SBET(m2g"l) Vp(cm3g"l) Dp(nm) 260.1 1.39 24.3 Ci4 4.25 981.3 0.6 2.45 243.1 1.18 18.9 Cl6 4.4 1064.6 0.66 2.6 noteworthy from the results in Figure 2 and Table 1 that the increase of the surfactant chain length causes the adsorption step at the position of p/po--0.2-0.5 to be shifted to higher relative pressure, but at the same time the adsorption step at the position of p/po=0.8-1.0 to be shifted to lower relative pressure. This suggests that an increase in primary framework pore size of BMS materials was accompanied concurrently by a decrease in its secondary framework pore size.
81 3.2. Effect of auxiliary structure director We consider another the effect of adding TMB into the reaction systems on the framework bimodal mesoporous structure of BMS materials. Figure 3 provides the X-ray diffraction patterns for BMS derivatives assembled from C~6 with TMB added as the auxiliary structure director. Structures formed from C~4 showed qualitatively equivalent diffraction features. The XRD patterns of as-synthesized BMS samples all contain a weak, relatively broad reflection at lower 2 0 angle. The qualitative form of the patterns is not affected by the presence of TMB. However, the positions of the intense reflection are dependent by the presence of TMB. It is worth noting that the degree of lattice contraction resulting from the calcination for the samples with TMB/TEOS molar ratio exceeding 0.58 is larger than that of other samples, this may indicate that a part of texture collapse has occurred. This can be confirmed from Figure 4, which provides corresponding N2 adsorption-desorption isotherms and pore size distribution
16000 12000 12000
f
8000
e
4000
C
f e
8000
d "
.......
0 0
C
4000
b
b
2
4
6
2-Theta
a
8
a
0 10
0
2
4
6
8
10
2-Theta
Figure 3. Powder XRD pattems of as-synthesized(A) and calcined(B ) BMS samples prepared using different TMB/TEOS molar ratio: a 0.065; b 0.194; c 0.322; d 0.451; e 0.58; f0.84. curves of BMS samples. Table 2 summarizes the relative structural parameters of series BMS samples. Clearly, the basal spacings represented by the main diffraction line are not correlated directly with the BJH primary pore sizes, even though the dl00 peaks of samples shift gradually to lower 2 0 angle and at the same time the primary mesopore sizes of BMS materials also increase gradually following the increase of TMB used in the reaction systems. The trend of bimodal mesoporous size adjustment resulting from the incorporation of TMB into reaction systems is similar with the results of increasing the surfactant chain length in the synthesis of BMS materials. The role of TMB as an auxiliary structure director on the primary mesopore size of BMS materials is also similar with its effect on the pore size of MCM-41 mesoporous materials, however, the degree of the primary pore size increase (ca. 1.0nm) is far smaller than that of MCM-41 materials. In contrast, it makes the secondary mesopore size of BMS materials contracted obviously (ca.6.4nm). After increasing TMB/TEOS ratio to exceed 0.58, the nitrogen adsorption isotherms of these samples vary significantly, showing that the
82
1200
A
.__J
800 400
I
0 1200 800
I
I
S
400 0
I
1200
I
I
C
m
~0
~D 9
<
800 4O0
S e~
0 1200
D
I
I
"
"
D
800 O
400
1200
E
i
800 400 0 1200 800 400
f
0
I
0
1
I,
0.2 0.4 0.6 0.8
1
Relative Pressure (P/Po)
10
100
1000
10000
Pore Size (A)
Figure 4. N 2 adsorption isotherms and corresponding pore size distribution curves for a series of BMS samples prepared at different TMS/TEOS mole ratio: A. 0.065; B. 0.194; C. 0.332; D. 0.451; E. 0.58; F. 0.84. structure has been affected. The sharp at p/po=0.8-1.0 decrease in nitrogen adsorption volume and shift of the step in nitrogen adsorption to lower P/Po imply that a large number of the secondary mesopores were destroyed and the pore size became smaller.
83 Table 2. Structural parameters for selected calcined BMS samples under study. Primary mesopore Sample A B C D E F
dloo(nm) SBET(mEg1) 4.25 4.56 4.51 5.26 4.55 4.80
1067.8 939.5 1106.9 937.6 1096.9 1138.3
Vp(cm3g"1) 0.69 0.66 0.76 0.71 0.87 0.85
Secondary mesopore
Dp(nm)
SBET(m2g "l) Vs(cm3g"1) Ds(nm)
2.88 3.15 3.27 3.20 3.28 3.50
270.2 260.9 288.8 271.9 \ \
1.05 0.95 1.07 0.87 \ \
17.0 15.8 14.6 12.5 \ \
The further experimental results show that BMS materials can be also synthesized using quaternary ammonium surfactant with alkyl chain length more than Cls, however, the chain length lower than C12 gives not a bimodal mesoporous structure but disordered mesostructure. The synthesis process of all BMS materials was completed in a short time and the viscosity of the reaction mixtures increased with time, and eventually set into jelly-like monoliths. These results suggest that under our synthesis conditions (pH ca.9.5), the relative rate of TEOS hydrolysis and condensation reactions may be almost equal[12], and, hence, the gel point is reached before the precipitation formed. After gelation, the effect of further extension reaction time on the products framework structure is negligible. In such a short reaction time, the surfactant micelles formed in the initial reaction mixtures may possess different size and shape, and the hydrolysis of TEOS and the condensation of the hydrolyzed products are incomplete, and thus the hydrolyzed SiO2 species are not enough to condense around every surfactant micelle. This may make some adjacent surfactant micelle interconnect and lead to the formation of mesopore framework of alternating hexagonal pore and stripe-like pore. The expansive micelles resulting from the increase of surfactant chain length or the addition of TMB into the reaction systems may require more hydrolyzed SiO2 species to ensure the formation of bimodal mesoporous framework structure in the prerequisite for two-grade mesopores expanded simultaneously. Obviously, at constant component concentration and thus hydrolyzed SiO2 species, it is inevitable results that the increase of primary mesopore size is accompanied by the decrease of secondary mesopore size. The further increase of TMB concentration may change the pH values of reaction systems and thus change the relative rate of TEOS hydrolysis and condensation reactions. The right proportion which is benefit for the formation of BMS materials between the hydrolyzed SiO2 species and surfactant micelles is destroyed. This may make the product's framework structure between some adjacent surfactant micelles susceptible to collapse during thermal treatment. As for the fact that the number of molar of ammonia in each reaction mixture was varied relying on surfactants alkyl chain length may be relevant with their different critical micelle concentration. Such a scenario would explain the pore size adjustment features of BMS materials, but further study are needed to fully understand the nature of the observed phenomena.
84 4. CONCLUSION The current study confirms that the methods used usually to control the pore size of MCM-41 mesoporous materials by adjusting the size of structure directing surfactant or the amount of auxiliary organic cosurfactant such as TMB added into the synthesis systems are also suitable for modifying the pore size distribution of BMS mesoporous materials. Because of the characteristic framework mesopore structure of our BMS materials, the increase of the primary framework mesopore size was accompanied simultaneously by the decrease of the secondary framework mesopore size, and the degree of increase of the primary mesopore size is far lower than that of decrease of the secondary mesopore size. These results suggest that the formation of bimodal mesoporous framework structure not only relies on an interaction between SiO2 species and the surfactant micelles, but also on a proportion of the hydrolyzed SiO2 species to surfactant micelles, and the pH adjustment of reaction systems and the relative rate of TEOS hydrolysis and condensation reactions resulting from the pH adjustment play a critical role in the synthesis of BMS molecular sieves. The controllability of bimodal mesoporous framework structure of BMS materials could make them more attractive for the practical applications. 5. ACKNOWLEDGMENTS This research was supported by the National Natural Science Foundation of China (Grant No.20073029). REFERENCES
1 P.T. Tanev, M. Chibeve and T.J. Pinnavaia, Nature, 368(1994)321. 2 R.M. Barrer, Hydrothermal Chemistry of Zeolites. Academic, London, 1982. 3 G. Guillemin, J.L. Patat, S. Foumie and M. Chetail, J.Biomed.Mater.Res., 21(1989)557. 4 J.S Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T.W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins and J.L. Schlenkere, J.Am.Chem.Soc., 114(1992) 10834. 5 C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli and J.S. Beck, Nature, 359 (1992) 710. 6 Q. Huo, D.I. Margolese, U. Ciesla, P. Feng, T.E. Gier, P. Sieger, R. Leon, P.M. Petroff, F. Shuth and G.D. Stucky, Chem.Mater., 6(1994)1176. 7 M. Kruk, M. Jaroniec and A. Sayari, J.Phys.Chem.B., 101 (1997)583. 8 Q. Huo, D.I. Margolese and G.D. Stucky, Chem.Mater., 8(1996)1147. 9 A. Sayari, P. Liu, M. Kruk and M. Jaroniec, Chem.Mater., 9(1997)2499. 10 X.Z. Wang, T. Dou and Y.Z. Xiao, Chem.Commun., 1998,1035. 11 X.Z. Wang, T. Dou, Y.Z. Xiao and B. Zhong, Studies in Surface Science Catalysis, 135 (2001)199. 12 E.J.A. Pope and J.D. Mackenzie, J.Non-Cryst.Solid., 87(1986) 185.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
85
A l c o t h e r m a l s y n t h e s i s o f large pore, high quality M C M - 4 8 silica Jihong Sun and Marc-Olivier Coppens* Chemical Reaction Engineering, DelftChemTech, Delft University of Technology, Julianalaan 136, 2628BL Delft, The Netherlands
A two-step method to synthesize high-quality MCM-48 with tunable pore size is presented. CTAB is used as a template and various alcohols are used as solvents in the second synthesis step. The samples were studied by means of XRD, SEM, and nitrogen sorption. This new synthesis method allows expanding the pore size from 2.0 nm to 2.5 nm by using ethanol as a solvent during the second synthesis step. The pore size enlargement is accompanied by an improvement of the pore size uniformity and the degree of order of the secondary MCM-48 material. The mechanism by which the pore size expansion occurs is explained in terms of the interactions between the solvent and the hydrophobic core and hydrophilic shell of the micelles formed by the template molecules.
1. INTRODUCTION The discovery of the M41S family of silicas with uniform and ordered mesopores has triggered a considerable research effort to synthesize porous materials with a tailored pore structure and long range structural order. Members of the M41S family are typically prepared via a liquid-crystal templating mechanism in which the templates consist of surfactant molecules ordered in different self-assembled arrays: hexagonal (MCM-41), cubic (MCM-48) or lamellar (MCM-50). MCM-41 contains a hexagonal array of one-dimensional pores; the diameter of its pores can be controlled between about 1.5 to 10 nm [1, 2]. The cubic MCM-48 (Ia3d), on the other hand, contains bi-continuous three-dimensional arrays of pore channels [3-5]. This facilitates molecular diffusion, which is useful in potential applications of MCM-48 in catalysis [6-9], adsorption [10] and separations [11 ], either by itself or as the starting material in the synthesis of multi-structured porous materials [ 12-14]. From this point of view, it is very interesting to synthesize well-ordered MCM-48 with a wide range of pore size.
To whom correspondence should be addressed. E-mail:
[email protected] Tel: +31-15-2784399 Fax: +31-15-2784452
86
However, MCM-48 is particularly difficult to synthesize due to the very sensitive synthesis conditions [ 15]. The conventional synthesis methods for expanding the pore size of MCM-48 proceed via a hydrothermal route, mainly changing the pH of the reaction medium [1, 2, 16], the catalyst [3], the reaction time [17, 18] and the temperature [19, 20]. Because MCM-48 easily looses its cubic structure when boiled in water even for a short time, several methods have been proposed to improve its hydrothermal stability. These include the addition of inorganic or organic salts to the synthesis medium [21-23], and the increase of the pore wall thickness via secondary synthesis [24] or post-synthesis hydrothermal restructuring [25]. It has recently been reported that post-synthesis treatment and tailoring the alkyl chain length of the cationic surfactant by using mixtures of cationic-anionic [27] and cationicneutral surfactants [28, 29] lead to an increased pore size of MCM-48. Meanwhile, gemini surfactants [30-32] added as swelling agents to the synthesis gel were found to favor the formation of MCM-48 with enlarged pores by adjusting the different surfactant chain lengths. Inspired by our earlier work on SBA-15 [33], we report on a new method via an alcothermal route to synthesize MCM-48 with considerably improved long-range structural order and increased pore size.
2. SYNTHESIS AND CHARACTERIZATION
2.1 Synthesis method The synthesis consists of two steps. In the first step, the surfactant cetyltrimethylammonium bromide (CTAB) was added to a mixture of deionized water and ethanol. Aqueous ammonia and tetra-ethyl orthosilicate (TEOS) were subsequently added at room temperature. The composition of the synthesis mixture was as follows: TEOS: CTAB: H20: ethanol: NH4OH = 1:0.4:174:54:12.5 (molar ratio), similar to the procedure described by Schumacher et al. [19]. After stirring the mixture continuously at room temperature, it became a white gel. This gel was filtered using a Bfichner funnel and repeatedly washed with distilled water. In the second step, the white gel was divided into two parts. One part was dried at 120~ for 3 hours, subsequently calcined in air by heating at a rate of l~ to 550~ and maintaining this temperature for 6 hours, leading to the "primary" MCM-48 material. Another part was immersed into a solution containing 5 wt% CTAB in various solvents ("base case": ethanol). The resulting gel was aged for 2 days in an autoclave at 100~ Finally, the product was filtered and washed with distilled water. After drying and calcination in a way similar to the procedure followed with the primary gel, a series of "secondary" MCM-48 materials was formed. 2.2 Characterization Powder X-ray diffraction (XRD) studies were performed using a Philips XRD spectrometer (PW1840) with CuK~l radiation, operating at 40 kV and 50 mA. Nitrogen adsorption/desorption isotherms were measured with a Micromeritics ASAP2000 sorption analyzer, utilizing the Barrett-Joyner-Halenda (BJH) method to evaluate the pore volume and pore size distributions for the desorption portion of the isotherm. Scanning electron
87 microscope (SEM) images were recorded using a Philips XL20. Samples were deposited on a sample holder with an adhesive carbon foil and sputtered with gold.
3. RESULTS AND DISCUSSION 3.1 Synthesis of large pore and high quality MCM-48
500 t
S}f
400
(420)(332)
Sample 2 ,o.o
(400) (321) ] J'l
o,=.,
/
300
o
200
I
1•/
0
2
4
6
8
10
20/~ Figure l XRD patterns of MCM-48
0.0
8.0
f'II
1~176 0
~......
4.0 .~
1.0
10.0 Pore diameter(nm)
t
!
1
1
1
0.2
0.4
0.6
0.8
1.0
Relative Pressure (P/P0) Figure 2 Nitrogen adsorption isotherms and corresponding pore size distribution of MCM-48
The XRD patterns for the calcined samples (Figure 1) show the characteristic cubic order of MCM-48 [1, 2]. The XRD pattern of the secondary material (sample 2), where ethanol was used as the solvent in the second step, shows a significantly increased intensity of the (211) peak, compared to the primary material (sample 1), as well as three higher order (220), (420) and (332) peaks. In addition, there are seldomly observed (321), (400), (422), and (431) peaks [15]. The higher peak intensities indicate that the second step extends the mesoscopic order [ 1, 2]. Meanwhile, the d2II spacing of sample 2 has increased from 3.1 nm to 3.4 nm, suggesting increased unit cell parameters. The nitrogen sorption isotherms and corresponding pore size distributions (Figure 2) indicate that the mesopore size increases from 2.0 nm to 2.5 nm, most likely by swelling of the organic structure-directing entities in the primary material [33]. The sharpness of the nitrogen condensation step (P/P0 = 0.2---0.4) and the well-defined XRD peaks provide strong evidence of the very high quality of this material. The hysteresis loop of sample 2 at a relative pressure P/P0 = 0.45~-0.9 is due to inter-particle porosity. The SEM image in Figure 4a reveals that sample 2 consists of agglomerated, irregularly shaped and partially cross-linked particles, about 0.8-1 pm in size, with macro-pores in between.
88 Table 1 Pore structure parameters of MCM-48 materials aa Sb Sample Solvent (nm) (mE/g) 1 2
Ethanol
7.8 8.3
1100 950
Vc
D d
(cma/g)
(nm)
He (nm)
0.75 0.73
2 2.5
1.5 1.4
a a = dhkl (h2+k2+12)l/2 is a cubic lattice parameter calculated from XRD. b S is the specific surface area obtained from nitrogen adsorption and desorption, c V is the specific pore volume, o D isthe mean pore diameter, e H = a/3.092 - D / 2 is the mean pore wall thickness.
Table 1 summarizes the textural characteristics of the primary and secondary MCM-48 materials. The highly ordered secondary MCM-48 (sample 2) has a pore wall thickness of approximately 1.4 nm, hardly changed from that in the primary MCM-48 (sample 1: around 1.5 nm). This indicates that the unit cell enlargement can be almost entirely attributed to an increase in pore size. Furthermore, the pore walls of sample 2 are thicker than those of typical high quality MCM-48 (around 0.8---1.0 nm) as reported in the literature [34]. To investigate the hydrothermal stability of the materials, 0.1 g of calcined secondary MCM-48 (sample 2) was boiled for up to 24 (211) hours in 100 ml of distilled water, using a Pyrex flask equipped with reflux condenser. XRD patterns were obtained after filtering and drying each boiled sample in an oven at "~'~ ~ L _ 12 hrs 150 ~ (Figure 3). Loss in XRD peak N 3 hrs intensity, as compared to that of the same sample before the boiling treatment, was used to judge the hydrothermal stability. Figure 3 Ohr shows that even after boiling in water for 24 hours, the XRD pattern of the secondary MCM-48 still shows the higher order (211) and (220) peaks, indicating long-range 0 2 4 6 8 10 mesoscopic ordering. The high hydrothermal 20/~ stability is a result of the thicker pore walls (1.4 nm) than for conventional MCM-48 Figure 3 XRD patterns of sample 2 (0.8-1 nm). However, after hydrothermal after boiling for different times in water. treatment, the XRD peak intensity is a little decreased compared to that without treatment in boiled water. This result suggests that the secondary MCM-48 (sample 2) using ethanol as solvent in the secondary synthesis step is of higher hydrothermal stability than the conventional MCM-48 (sample 1), which easily loses its cubic structure after boiling in water for a short period of time (< 8 hours). Therefore, the pore size enlargement is not accompanied by a loss in hydrothermal stability.
89 3.2 The effect of the type of alcohol on the pore expansion
Figure 4 SEM images of secondary MCM-48 materials, prepared using different solvents in the second synthesis step: a: ethanol; b: 1-hexanol, c: benzene
The XRD and nitrogen sorption results show that ethanol acts as a swelling agent: addition of ethanol in the second synthesis step apparently expands the CTAB liquid crystal within the pores of the MCM-48 primary gel particles. This is similar to what we recently observed for the swelling of the P-123 template in an analogous two-step synthesis of highly ordered SBA-I 5 [33]. Figure 5 shows the XRD patterns of samples 2-5 prepared using alcohols with an increasihgly long alkyl chain as solvents in the second synthesis step. While the diffractogram of sample 2, for which ethanol was used as a solvent, shows 8 intense reflections (also shown in Figure 1), the diffractograms of samples 3-5, using 1-propanol, 1butanol and 1-hexanol as solvent respectively, show a gradual shift of the (211) peak to low angles, a further broadening and weakening of this peak, and a disappearance of all other peaks in the region 28 = 3-10 ~ This indicates that the swelling action of these longer alcohols leads to extensive structural degradation and loss of order. When non-polar benzene is used as a solvent, the template dissolves and the ordered structure of the primary gel collapses: sample 6 exhibits the lowest degree of structural ordering of all samples. The SEM images show that the particle size of sample 4, for which hexanol was used as a solvent, is around 0.6 ktm (Figure 4b), which is smaller than that of sample 2 (Figure 4a), where ethanol was used (0.9 pm). When benzene is used (Figure 4c), the individual particle structure largely disappears, as the particles agglomerate.
90 The above results indicate that, in contrast to ethanol (sample 2), both benzene (sample 6) and alcohols with longer alkyl chains (samples 3-5), are unsuitable solvents in the preparation of large pore MCM-48. The effects of different alcohols on the phase behavior and microstructure I can be explained in terms of polarity and affinity to the different segments of the cubic liquid crystal structure. It is well known that ionic surfactant CTAB dissolved in water can spontaneously associate to form =~ micelles, with the hydrophobic block ~, localized in the micelle core and the hydrophilic block forming a corona (shell) around the core [1, 2]. Since ethanol is polar and completely miscible with water, it may participate 0 2 4 6 8 10 in the formation of the interface between the hydrophobic and the 2 0/o hydrophilic domains [35]. On the other hand, ethanol has more Figure 5 XRD patterns of the secondary MCM-48 tendency than water to penetrate into prepared by using different solvent. the hydrophobic region of the sample 2: ethanol; sample 3: 1-proapnol; micelles, and hereby increase the sample4: l-butanol;sample5: 1-hexanol; volume of the hydrophobic core. sample6:benzene Both the core and the corona of the cubic liquid crystal phase formed during the first synthesis step are swollen in ethanol [36], resulting in an improvement of its degree of order, as evidenced from the XRD patterns in Figure 1. The physical properties of 1-propanol are similar to those of ethanol, while those of 1butanol differ: it is less soluble in water (up to -7.5 wt % soluble in water at 25 ~ [37]. The XRD patterns indeed indicate that the structural order is largely lost (see Figure 5), while the position of the (211) peak is shifted to a lower angle, due to the expansion of the liquid crystal structure with an increased alkyl chain length. This is different from what we observed for SBA-15, where the primary hexagonal order was maintained upon enlarging the pores using a similar treatment [33]. This may be due to the lower stability of the cubic liquid crystal phase [38], even in propanol. l-Hexanol greatly differs in its properties from ethanol and propanol" it is polar but insoluble in water [37]. Because of this, it almost exclusively enters the non-polar hydrophobic domain of the CTAB liquid crystal and expands it, but does not swell the hydrophilic domain. As a result, the cubic phase becomes unstable, and the MCM-48 structure collapses (sample 5). Treatment with benzene as a solvent, being non-polar and immiscible with water, leads to a complete disappearance of the (211) peak in the XRD pattern (see Figure 5: sample 6). The mesopore channels formed in the first synthesis step collapse, dueto a very strong interaction of benzene with the hydrophobic core of the micelles formed by CTAB, which is dissolved. ._
r~
91 This results in a destruction of most of the liquid crystalline structure, so that a disordered amorphous material is formed. As follows from this study, the relation between the CTAB phase behavior and the solvent polarity indicates that the latter has a significant effect on the cubic liquid crystal and its templating action.
4. CONCLUSION It was shown that restructuring of a primary MCM-48 gel using CTAB in ethanol yields a secondary MCM-48 with larger pores and a higher degree of order, while maintaining thick pore walls around 1.4 nm, which increases the hydrothermal stability. From nitrogen sorption, it was determined that the surface area of the secondary MCM-48 materials is around 950 m2/g and the average pore size increases from 2.0 nm to 2.5 nm. The XRD characteristics displayed eight well-resolved diffraction peaks corresponding to the cubic Ia3d structure, when ethanol is used as a solvent during the second synthesis step, which implies that the structure of the secondary MCM-48 is highly ordered. However, the degree of order of the secondary materials sharply decreased with increased carbon number of the alkanol solvent from 2 to 6 carbons. The expansion mechanism of MCM-48 was briefly discussed in terms of the polarity of the alcohol and its affinity to the different segments of the cubic liquid crystal structure formed by CTAB during the first synthesis step. Alcohol may permeate into the hydrophobic core and/or hydrophilic shell of micelles, and thereby induces a structural rearrangement of the liquid crystal phase. Non-polar benzene has the tendency to destroy the liquid crystals, because it is a good solvent for CTAB. Further studies are required to investigate other synthesis parameters such as the acidity, synthesis period and temperature during the second synthesis step. ACKNOWLEDGEMENT We would like to thank P. Boeser for measuring the nitrogen adsorption isotherms.
REFERENCES
1. 2.
3.
4. 5. 6. 7.
C . T . Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli, J. S. Beck, Nature, 359 (1992) 710. J.S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T.-W. Chu, D. H. Olson, E. W. Sheppard, S. B. McCullen, J. B. Higgins, J. L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. A. Monnier, F. Schuth, Q. Huo, D. Kumar, D. Margolese, R. S. Maxwell, G. D. Stucky, M. Krishnamurty, P. Petroff, A. Firouzi, M. Janicke, B. F. Chmelka, Science, 261 (1996) 1299. V. Alfredsson, M. W. Anderson, Chem. Mater., 8 (1996) 1141. M.W. Anderson, Zeolites, 19 (1997) 220. A. Corma, Chem. Rev., 97 (1997) 2372. M.S. Morey, J. D. Bryan, S. Schwarz, G. D. Stucky, Chem. Mater., 12 (2000) 3435.
92 8. 9. 10. 11. 12. 13. 14. 15. 16. 17.
18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30. 31. 32. 33. 34. 35. 36. 37. 38.
M. Kruk, M. Jaroniec, R. Ryoo, J. M. Kim, Chem. Mater., 11 (1999) 2568. R.H. Hall, C. E. Fowler, B. Lebeau, S. Mann, Chem. Commun., (1999) 201. C.M. Bambrough, R. C. T. Slade, R. T. Williams, S. L. Burkett, S. D. Sims, S. Mann, J. Colloid Interface Sci., 201 (1998) 220. C. Thoelen, K. van de Walle, I. F. J. Vankelecom, P. A. Jacobs, Chem. Commun., (1999) 1841. R. Ryoo, S. H. Joo, S. Jun, J. Phys. Chem. B, 103 (1999) 7743. J. Lee, S. Yoon, T. Hyeon, S. M. Oh, K. B. Kim, Chem. Commun., (1999) 2177. R. Ryoo, S. H. Joo, S. Jun, T. Tsubakiyama, O. Terasaki, Stud. Surf. Sci. Catal., 135 (2001) 07-0-01. A. Sayari, J. Am. Chem. Soc., 122 (2000) 6504. J. Xu, Z. Luan, H. He, W. Zhou, L. Kevan, Chem. Mater., 10 (1998) 3690. J. C. Vartuli, K. D. Schmitt, C. T. Kresge, W. J. Roth, M. E. Leonowicz, S. B. McCullen, S. D. Hellring, J. S. Beck, J. L. Schlenker, D. H. Olson, E. W. Sheppard, Chem. Mater., 6 (1994) 2317. M.L. Pena, Q. Kan, A. Corma, F. Rey, Micro. Meso. Mater., 44-45 (2001) 9. K. Schumacher, M. Grun, K. K. Unger, Micro. Mater., 27 (1999) 201. L.Z. Wang, J. L. Shi, J. Yu, W. H. Zhang, D. S. Yan, Mater. Lett., 45 (2000) 273. R. Ryoo, S. Jun, J. Phys. Chem. B, l01 (1997) 317. J.M. Kim, S. Jun, R. Ryoo, J. Phys. Chem. B, 103 (1999) 6200. D. Das, C.-M. Tsai, S. Cheng, Chem. Commun., (1999) 473. R. Mokaya, J. Phys. Chem. B, 103 (1999) 10204. S. Jun, J. M. Kim, R. Ryoo, Y.-S. Ahn, M.-H. Han, Micro. Meso. Mater., 41 (2000) ll9. F. Chen, F. Song, Q. Li, Micro. Meso. Mater., 29 (1999) 305. R. Ryoo, S. H. Joo, J. M. Kim,, J. Phys. Chem. B, 103 (1999) 7435. M. Kruk, M. Jaroniec, Chem. Mater., 12 (2000) 1414. P. van der Voort, M. Mathieu, F. Mees, E. F. Vansant, J. Phys. Chem. B, 102 (1998) 8847. M. Benjelloun, P. van der Voort, P. Cool, O. Collart, E. F. Vansant, Phys. Chem. Chem. Phys., 3 (2001) 127. M. Mathieu, E. van Bavel, P. van der Voort, E. F. Vansant, Stud. Surf. Sci. Catal., 135 (2001) 06-0-04. M. Morey, S. O'Brien, S. Schwarz, G. D. Stucky, Chem. Mater., 12 (2000) 898. J.H. Sun, J. A. Moulijn, J. C. Jansen, T. Maschmeyer, M.-O. Coppens, Adv. Mater., 13 (2001) 327. K. Schumacher, P. I. Ravikovtch, A. D. Chesne, A. V. Neimark, K. K. Unger, Langrnuir, 16 (2000) 4648. R. Ivanova, P. Alexandridis, B. Lindman, Colloids and Surfaces A., 183-185(2001), 41. Q. Huo, D. I. Margolese, G. D. Stucky, Chem. Mater., 8 (1996) 1147. D.R. Lide (ed), Handbook of chemistry and physics (81st), CRC Press, 2000. P. Alexandridis, U. Olsson, B. Lindman, Langmuir, 14 (1998) 2627.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
93
Studies o f M C M - 4 1 obtained from different sources o f silica Icaro S. Paulino and Ulf Schuchardt* Instituto de Quimica, Universidade Estadual de Campinas, P.O. Box 6154, 13083-970 Campinas-SP, Brazil.
An efficient and simple method has been used to synthesize MCM-41 at room temperature under stirring. The mesoporous materials were obtained using three different silica sources, tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), tetrapropoxysilane (TPOS), ammonium hydroxide and cetyltrimethylammonium bromide (CTMABr) as template, in various reaction times The route of the synthesis was monitored by X-ray diffraction (XRD) which showed that a highly ordered mesoporous material was obtained after just 15 min. The effect of the silica source on the properties of the MCM-41 samples obtained is also discussed wing nitrogen sorption and X-ray diffraction
1. INTRODUCTION The synthesis of MCM-41 type mesoporous materials has been the subject of intensive research in the last years. Since the discovery of the M41S family of mesoporous materials in the beginning of the 90s [1-3] intensive studies have been conducted by various research groups with the objective to understand the synthesis mechanism as well as the role of synthesis (time, pH, temperature, surfactant/silica ratio, choice of the surfactant kind and morphofogy control) on the formation of the mesoporous structure. MCM-41 exhibits a hexagonal array of one-dimensional mesopores, whose diameters can be tailored form 1.5 to 10 nm with a narrow pore-size distribution. The pore walls are composed of amorphous silica, as indicated by X-ray diffraction measurements. The structure of this material is shown schematically in Figure 1.
Figure 1. Schematic representation of the hexagonal array of one-dimensional mesopores of MCM-41.
94 The discovery of this new class of molecular sieves allowed the development of new heterogeneous catalysts. Besides the easy access to the channels, MCM-41 shows the possibility of isomorphic exchange in the structure, leading to the formation of materials with acid, basic or redox properties. The incorporation of various metals into the MCM-41 framework has granted them catalytic properties, allowing their use in hydroxylation and dehydrogenation of.aromatic compounds [4,5], epoxidation of unsaturated fatty esters [6] and oxidation of bulky organic molecules with aqueous H202 or tert-butyl hydroperoxide (TBHP) as oxidant [7,8]. Due to the open structures and large pore-size, together with their adsorption properties, MCM-41 has been used as support of metallocenes to generate catalysts for heterogeneous phase polymerization [9,10]. The physicochemical properties of MCM-41, as pore size distribution, hydrothermal stability, pore arrangement and silanol content depend very much on synthesis methods, which allow the preparation of a wide range of materials with different pore sizes, surface areas and numbers of peaks in XRD experiments [ 11 ]. Differences in preparation methods also may result in materials with different wall structures, but some of them show structural instability. In this work we report a simple and reproducible synthesis of MCM-41 type mesoporous materials via an efficient and rapid method, at room temperature, using three different silica sources, tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), tetrapropoxysilane (TPOS). The effect of the silica source upon properties of the MCM-41 samples are also discussed using nitrogen sorption and X-ray diffraction.
2. EXPERIMENTAL
2.1. Synthesis Tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), tetrapropoxysilane (TPOS), cetyltrimethylammonium bromide (CTMABr) were purchased from Aldrich and aqueous ammonia (25 wt. %) was obtained from Baker. All chemicals were used asreceived. Mesoporous molecular sieves were synthesized at room temperature from a mixture of appropriate quantities of CTMABr added as a solution in aqueous NHaOH. The silica source, TMOS, TEOS or TPOS, was then added to obtain a final mixture with the following molar composition: 1 Si : 33 NHaOH : 330 1-120:0.12 CTMABr. The mixture was kept under stirring for 15 min up to 20 h. The obtained solid was separated by filtration, dried at 373 K and finally calcined at 813 K for 4 h under a flow of nitrogen and subsequently for 6 h under a flow of synthetic air (heating rate 1 K minl).
2.2. Characterization 2.2.1. Powder X-ray diffraction (XRD) The X-ray diffractograms were recorded on a Shimadzu XRD6000 diffractometer using Cu-Kct radiation generated under 40 kV, 30mA. Diffraction data were recorded between 1.5 ~ and 10~ (20) at a interval of 0.02 ~ with a scanning rate of 1~ min 1. The slits used were 0.5 ~ 0.5 ~ 3 mm for divergence, scattering, reception, respectively.
2.2.2. Infrared Spectroscopy (IR) The FT I.R. spectra were obtained on a Perkin Elmer 1600 M-80 spectrometer between 400 and 4000 cm ~ in the transmission mode, using KBr pellets. Sixteen scans were accumulated at a 4 cm 1 resolution.
95
2.2.3. Thermogravimetric Analysis (TGA) The thermogravimetric analyses were performed under a nitrogen flow of 100 mL min l on a DuPont 951 TGA thermobalance between 293 and 1,273 K, using a heating rate of 10K mln . 9
-|
2.2.4. Pore-structure Analysis (ASAP) Adsorption and desorption isotherms for nitrogen were obtained at 77 K using a Micromeritics analyzer ASAP 2010. The samples were degassed at 423 K for 12 h before measurements were performed. Specific surface area values were obtained using the BET (Brunauer-Emmett-Teller) equation 9
2.2.5. Electron Microscopy (SEM) Scanning electron microscopy was performed on a DSM940A Zeiss microscope or on a JSM-T300 Jeol microscope, under an accelerating voltage of 20 kV.
3. RESULTS AND DISCUSSION The FT-IR spectra of the MCM-41 materials show bands between 1400 and 450 cm -~ due to fundamental vibrations of the framework [ 12], a band in-1650 cm l relative the O-H bond deformation. The spectra also presented a large band around 3000 cm l, relative to O-H stretching, which impedes the visualization of the characteristic bands of silanol groups [13]. We also observe the bands at 1489, 2844 and 2916 cm -1 due to the surfactant, which disappears upon calcination. The thermogravimetric analysis reveals a weight loss of about 12 % that is due to water desorption (< 200 ~ and silanol groups condensation (> 200 ~ The characteristic structural element of MCM-41 is a hexagonal array of the pores. The powder X-ray diffraction (XRD) patterns obtained from the non-calcined MCM-41 is typical of a well ordered structure and shows four Bragg peaks at low reflection angles between 2 and 7~ (20) that can be indexed to a hexagonal lattice as (100), (110), (200) and (210). The XRD patterns indicate that there are no crystalline phases present, because no reflections at higher angles are observed. However, as suggested by Cheng et al. [ 14], the term crystalline can be used only with respect to the periodic array of channels that represent the single element of order in the material. We performed some studies varying the reaction time to verify the structural development of MCM-41 with time. In studies of reaction times, Ortlam et al. [ 15] compared the temporal development of the X-ray reflection intensities of as-synthesized and calcined MCM-41 materials. They observed that the hexagonal structure of MCM-41 may be formed after reaction times of about lh at 104~ and that 90% of the hexagonal channel arrangement is formed after 5-6 h, whereas the fully developed mesopore structure requires 72 h. The XRD patterns obtained in this work from non-calcined MCM-41 recorded after different times are shown in Figure 2. We can observe that the structural arrangement of MCM-41 is formed after 15 min and maintained with prolonged reaction times. A rapid hydrolysis process of TMOS can explain this behavior TEOS and TPOS, assisted by the controlled pH and an efficient condensation under these synthesis conditions. However, these materials had demonstrated a very poor thermal stability, since the structure collapsed during the calcination process 9 Only crystallization times higher than 2 h allow the formation of MCM-41 that presented high thermal stability. Another feature of these diffractograms is the increasing of peaks intensity with reaction time and their shift to lower 20 values, indicating an growth of the unit cell.
96
However, when the MCM-41 samples were submitted to the calcination process, the peak intensities of the XRD patterns decrease and the 20 positions shift to a higher value indicating a contraction of the lattice. This process is caused by the removal of the surfactant from the channels, and subsequent condensation of silanol groups on the walls. We can observe the disappearance of peak (210); this is probably due to a reduction of the order of the structure. The XRD patterns for the MCM-41 as-calcined are shown in Figure 3. The observed 20 angles, the relative Miller indices (hkl) and the unit cell parameter ao calculated by linear regression of equation (1) are listed in Table 1. ao2= 4d2(h 2 + k 2 + hk)/3
(1)
(100)
20h 2h lh 0.5h 0.25 h
;
'
~
'
~
'
;
'
~
'
1'0'
1'2
2O Figure 2. XRD patterns of the as-synthesized samples with different reaction times, using TPOS as silica source.
TPOS TEOS
0)
TMOS
;
'
~
'
~
'
;
'
~
'
1'0
2O Figure 3. XRD pattems of the calcined MCM-41 using TMOS, TEOS and TPOS as silica source.
97
Table 1 X-ray data of MCM-41 synthesized with TMOS, TEOS or TPOS as silica sources. Source of silica TMOS
TMOS-calc.
TEOS
TEOS-calc
TPOS
TPOS-cal
hkl
Observed 20 (o)
dhkl (nm)
100 110 200 210 100 110 200 210 100 110 200 210 100 110 200 210 100 110 200 210 100 110 200 210
2.26 3.86 4.46 5.86 2.50 4.28 4.96
3.91 2.29 1.98 1.54 3.53 2.05 1.78
2.20 3.80 4.38 5.80 2.44 4.22 4.86
4.01 2.32 2.02 1.52 3.62 2.09 1.82
2.16 3.76 4.34 5.72 2.42 4.18 4.84
4.09 2.35 2.03 1.54 3.65 2.11 1.83
Unit cell parameter (XRD) ao (nm) 4.50
4.08
4.63
4.17
4.71
4.21
It is important to observe that an increase of alkoxy group shifts of the 20 positions to smaller values, and consequently lager unit cell parameters are obtained. After the calcination process of the samples an expected contraction of 9 % (Aao = 0.4 - 0.5 nm) of the unit cell parameter was observed. This unit cell contraction is near to that observed by Cai et al. [ 16] in similar synthesis conditions. Nitrogen adsorption measurements were carried out for the calcined samples as another method to confirm the highly ordered MCM-41 structure. The adsorption and desorption isotherms of nitrogen of each sample show the typical type IV isotherm, as defined by the International Union of Pure and Applied Chemistry (IUPAC) [ 17]. However, the isotherm obtained for MCM-41 synthesized using TMOS as silica source can be considered type I, since it presents very small inflection characteristics of capillary condensation processes. The nitrogen adsorption isotherms obtained at 77 K for calcined MCM-41 are shown in Figure 4. We observe three stages of nitrogen adsorption and desorpfion in the isotherms. The adsorptions at very low relative pressure, p/po, correspond to monolayer-multilayer adsorption on the pore walls with no pressure transitions and no inflection points indicating complete absence of micropores [ 18]. The increase of the absorbed volume at low pressures is followed by a steep with an inflection point at intermediate relative pressures, which is due to capillary condensation inside the mesopores. The last stage is a plateau at high relative pressures
98 associated with multilayer adsorption on the extemal surface of the crystals [19]. This indicates that the mesoporous were completely filled. The fact that inflections of the isotherm (TPOS) are sharper indicates that the MCM-41 synthesized with TPOS presentes a narrow pore size distribution. This can be related to the fact that TPOS is hydrolyzed more slowly in comparison to TEOS and mainly to TMOS. 700 600
TPOS ,.0~9~0~4--0~- 0 --0--0--0 - - 0 - 0 ~ 0
500 E
~
TEOS
400 300-
< 200"6 > 100-
~~"
~
c)_..~o
o
TMOS /o--9--9--2~-P~' +
-I-
T
[__~ Adsorption DesorptionI
0
0,0
'012'014 0',6 ' 0',8 RelativePressure(P/Po)
'
1,0
Figure 4. Nitrogen adsorption isotherms obtained at 77 K of MCM-41 calcined using TMOS, TEOS and TPOS as silica source. An important characteristic of nitrogen adsorption is that the specific pore volume, specific surface area and average pore diameter become larger with increasing carbon chain length of the alkoxy group as shown in Table 2. The MCM-41 synthesized using TMOS as silica source, presents the smallest specific pore volume, specific surface area and average pore diameter. On the other hand, the MCM-41 synthesized using TPOS as silica source, presents the largest specific pore volume, specific surface area and average pore diameter. The Brunauer-Emmett-Teller (BET) method [20] was used to calculate the specific surface area. Considering that the MCM-41 channels are cylindric, the diameters D of the mesoporous were calculated following the equation 2 given by Gurvitsch method: D4v/S = 4 Vmes/SBET
(2)
where Vines is the mesoporous volume estimated from the N2 adsorption isotherm and Sser is the BET surface area. The most used method to calculate the pore size distribution is based on the BarrettJoiner-Halenda (BJH) model [21 ]. However, we did not apply this model to calculate average pore diameter due to an underestimation of the pore diameter. This is occurred due to the instability of the liquid nitrogen meniscus inside the mesopores. The wall thickness of the MCM-41 was calculated by the difference between unit cell parameters ao, determined by X-ray diffraction, and the pore diameter (eq. 2) obtained by equation 3. e:ao-D
(3)
99 The values of wall thickness are in agreement with the literature, except for MCM-41 synthesized with TMOS that presented e = 1.83 nm. However, this value is only approximation, since there is no type IV isotherm. We therefore must be cautious with the values of e obtained using different analysis techniques. Same of the properties of the calcined MCM-41 samples (prepared by the use of different tetraalkoxisilane) obtained by nitrogen sorption, X-ray diffraction and density analysis are shown in Table 2. Table 2 Properties of the MCM-41 samples as-calcined prepared by use of different tetraalkoxisilane obtained by nitrogen sorption and X-ray diffraction. Source of silica
Specific pore volume
Specific surfacea r e a
c m 3 g-i
m 2 g-i
0.39 0.72 0.84
685 1002 1127
TMOS TEOS TPOS
Average pore diameter(N2sorption) n m 2.25 2.86 2.99
Wall thickness (nm)
Density (g cm_3)
1.83 1.31 1.22
2.00 1.96 1.81
Scanning electron microscopy was used to determine the particle size, particle morphology and the particle size distribution of the synthesized MCM-41. The particle size of all samples range from 0.5 gm to 2.0 gm with an average size of 1.1 pan. While the particles of MCM-41 synthesized with TEOS and TPOS presents a morphology more defined, the MCM-41 synthesized with TMOS presents fused particles. This can to be attributed to the fast hydrolysis process of TMOS, which may cause the particle coalescence. The scanning electron micrographs are shown in Figure 5.
(a)
(b)
(c)
Figure 5. Scanning electron micrographs of MCM-41 as-calcined using (a) TMOS, (b) TEOS and (c) TPOS as silica source.
4. CONCLUSIONS In this work we report the synthesis of MCM-41 type mesoporous materials via an efficient and rapid method at room temperature using the three different silica sources, TMOS, TEOS and TPOS. We observe that the structural arrangement of MCM-41 is formed after 15 min, but only after crystallization times of more than 2 h MCM-41 with high thermal stability is formed. We observe that with the the increase of chain alkoxy group a higher unit cell parameter, specific surface area, specific pore volume and average pore diameter is obtained.
100 Particularly, it appears clear that the use of TPOS produces an improvement in the structure of MCM-41. Because of these characteristics, the MCM-41 is an excellent support for various 9 catalysts, where are used in transesterification, oxidation and polymerization reactions of olefins, in our research group.
5. ACKNOWLEDGEMENTS The authors thank FAPESP and CNPq for financial support for this work (grant number 99/02649-5) and Profs. Mafia do Carmo Gongalves and Heloise de Oliveira Pastore for assistance.
REFERENCE
1. T. Yanagisawa, T. Shimizu, K. Kuroda e C. Kato, Bull. Chem. Soc. Jpn., 63 (1990) 988. 2. J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.P. Schmitt, C.T.W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins e J.L. Schlenker; J. Am. Chem. Soc. 114 (1992) 10834. 3. C.T. Kresge, M.E. Leonowicz, J.C. Vartuli and J.S. Beck, Nature, 359 (1992) 710. 4. C. Lee, W. J. Lee, Y. K. Park, S. Park, Catalysis Today, 61 (2000) 137. 5. S. Wong, H. Lin, C. Mou, Applied Catalysis A: General, 198 (2000) 103. 6. M.A. Camblor, A. Corma, P. Esteve, A. Martinez and S. Valencia, Chem. Commun., 795 (1997). 7. W.A. Carvalho, P. B. Varaldo, M. Walau and U. Schuchardt, Zeolites, 18 (1997) 408. 8. W.A. Carvalho, M. Walau and U. Schuchardt, J. Mol. Catal. A, 144 (1999) 91. 9. Y.S. Ko, T. K. Han, J. W. Park e S. I. Woo, Macromol. Rapid Commun., 17(1996) 749. 10. I. S. Paulino, A. P. de Oliveira Filho, J. L. de Souza and U. Schuchardt, Stud. Surf. Sci. Catal., 130 (2000) 929. 11. S. Biz and M. L. Occelli, Catal. R e v . - Sci. Eng., 40 (1998) 329. 12. G. Cent, S. Parathoner, F. Trifir6 A. Aboukais, C. F. Aissi and M. Guelton, J. Phys. Chem., 96 (1992) 2617. 13. M. D. Alba, Z. Luan and J. Klinowski, J. Phys. Chem., 100 (1996) 2178. 14. C-F. Cheng, W.Zhou, D. H. Park, J. Klinowski, M. Hargreaves and L. F. Gladden, J. Chem. Soc., Faraday Trans. 93 (1997) 359. 15. A. Ortlam, J. Rathousky, G. Schulz-Ekloff and A. Zukal, Microporous Mater., 6 (1996) 171. 16. Q Cai, W-Y Lin, F-S Xiao, W-Q Pang, X-H Chen and B-S Zou, Microporous Mesoporous Mater. 32 (1999) 1. 17. K. S. W. Sing, D. H. Everett, R. A. Haul, L. Moscou, R. A. Pierotti, J. Rouquerol and T. Siemieniewska, Pure Appl. Chem., 57 (1985) 603. 18. S. Storck, H. Bretinger and W. F. Maier, Appl. Cat. A: General, 174 (1998) 137. 19. P. J. Branton, P. G. Hall and K. S. W. Sing, J. Chem. Soc., Chem. Commun., 1257 (1993). 20. S. Brunauer, P. H. Emmett and E. Teller, J. Am. Chem. Soc., 59 (1937) 1553. 21. E. P. Barrett, L. G. Joyner and P. P. Halenda, J. Am. Chem. Soc., 61 (1951) 373.
b t U d l e s i n b u r t a c e :::iclence a n a t s a t a l y s l s 1/41
A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
Synthesis and characterization of hexagonal hydrothermal restructuring method
101
mesoporous
materials
using
Kyoung-Ku Kang and Hyun-Ku Rhee School of Chemical Engineering and Institute of Chemical Processes Seoul National University, Kwanak-ku, Seoul 151-742, Korea
Pure siliceous MCM-41 samples were prepared by the usual hydrothermal synthesis method and also by the hydrothermal restructuring method. The hydrothermal restructuring procedure was carried out by the pH control and the rehydrothermal treatment. The restructuring method gave almost 90% of yield of calcined Si-MCM-41 on the basis of the weight of silica in the reaction mixture. All the samples were characterized by using X-ray diffraction (XRD), TEM, and N2 physisorption. The XRD patterns of all the samples exhibited the well-defined reflections and the (100) reflection of the restructured samples showed no shift after calcination because the wall of Si-MCM-41 was densely packed by the restructuring procedure. During the restructuring procedure, the values of d-spacing and unit cell parameter of Si-MCM-41 were increased. TEM analysis revealed that the restructured sample has a highly ordered hexagonal array. According to the N2 physisorption results, the restructured samples possessed a small pore size compared with that of the sample without being treated. Both the pH control and the rehydrothermal treatment have exercised influences on the structure of Si-MCM-41.
1. INTRODUCTION Mesoporous materials (M41S) have been synthesized by researchers at Mobil in recent years [1]. These materials consist of three different types of structure; hexagonal arrayed structure of MCM-41, 3D arrayed structure of MCM-48 and lamellar arrayed structure of MCM-50. These mesoporous materials exhibit unique characteristic properties. First, they possess a uniform pore size in the nano range (3-10 nm). Secondly, it is easy to control the pore size by using alkyl chain structure directing agents of different lengths [1 ] or micelle swelling agent (like trimethylbenzene) [2]. Mesoporous molecular sieves have also attracted much attention because of their unique properties [1]. Since the discovery of mesoporous materials, these materials have been applied as catalyst supports, adsorbents, column materials for separation, and hosts for large molecules [3]. The research interest in this field has been focused on their synthesis mechanism, development of synthesis procedure such as morphology control, enhancement of stability, characterization, synthesis of new materials based on MCM-41 synthesis concept, and technical applications [1,3-5]. Among them, the development of synthesis method is considered to be one of the most important subjects.
102 The aim of this work is to improve the textural properties of Si-MCM-41. To achieve this goal, we have developed a hydrothermal synthesis using pH control and rehydrothermal treatment and investigated the effect of hydrothermal restructuring method by applying various analysis techniques. As a result, it is found that both the rehydrothermal treatment and forced pH control result in an increase in the wall thickness. Therefore, the hydrothermal restructuring method is proven effective to improve the structural properties of mesoporous materials.
2. EXPERIMENTAL
2.1 Synthesis The Si-MCM-41 sample was prepared by using the usual hydrothermal synthesis method at 383 K. A sodium silica solution was prepared by combining aqueous NaOH solution with Ludox HS-40 (SiO2 40 wt% colloidal silica in water, Dupont). The resulting mixture was heated under stirring until clear. The template solution was then prepared with distilled water and cetyltrimethylammonium bromide (CTMABr) at 303K in an isothermal water bath. The sodium silicate was slowly added to the template solution under vigorous stirring. The composition of the resultant gel was SiO2 : 0.25 CTMABr : 0.7 Na20 : 60 H20. The gel obtained was stirred at room temperature for 1 h. The CTMA-silicate mixture was heated in an autoclave reactor without stirring to 383 K for 24 h. The precipitated product was hotfiltered, washed with distilled water and dried in an oven at 373 K overnight. The product was calcined in air at 823 K for 5 h by using a muffle furnace.
2.2. Hydrothermai restructuring method The restructured Si-MCM-41 samples were prepared with SiO2 : 0.25 CTMABr : 0.7 Na20 : 60 H20 by following the same mixing procedure as before and the hydrothermal reaction proceeded for 1 day. The value of pH was monitored by a digital pH meter. The reaction mixture was then cooled to room temperature, and the pH of the mixture was adjusted to -8 using strong acidic solution under vigorous stirring for more than 1 h. The resultant gel became homogeneous white solution. After stirring for lh, the pH of the mixture was adjusted to -10 using thick NaOH solution under vigorous stirring for 1 h and distilled water of 1'0 % by volume was added under vigorous stirring. This mixture was heated again at 383 K for 24 h. The pH adjustment and subsequent heating were repeated two more times. Finally, the solid product was hot-filtered, washed and dried in an oven at 373 K for overnight. The product was calcined in air at 823 K for 5 h by using a muffle furnace. 2.3. Characterization The yield of Si-MCM-41 is defined by the ratio of the weight of pure silica (SiO2) phase to the total weight of SiO2 in the reaction mixture. The weight of Si-MCM-41 was measured after calcination process. The phase identification of the solids were performed by using Xray diffractometer (Rigaku, D/MAX-II A) equipped with an Ni-filtered monochromatic Cu Ka (;~=1.54056 A) radiation from a tube at 30 kV and 40 mA. The morphology of the samples was examined by TEM (Jeol model JEM-2000EXII). The specific surface area and the average pore diameter were determined by nitrogen physisorption with the BET method at the liquid nitrogen temperature using a Micrometrics ASAP 2010 automatic analyzer.
103
Usual Synthesis Procedure ..
,"*
:
I
. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
] #
.....................................................................................
] "**,
Cooling to room temperature, pH control with acid to about 8
1 "
IL :
~
9
Stirred at room temperature for 1 h
ID4'I, i l l l l l l i
:
~i pH control with NaOH solution and addition of water
,millER
~]
:"
:...: :.......:....:.::......:....w :.:E.: :: :.: :...
- ..................... Kept in a convection oven maintained at 383 K lEniN
: 9
IL
: ...: :.: :..:..: :.:.....:: :
]
....................
:
:.
pH control
ii l l l l l l l l l l l l l l , I l l i l l
i
~ rehydrothermal " treatment
Ilillll,llllIIIlllllllllllllllllllllllllll*
Filtration, washing and drying at 373 K for 24 h i
.....Calcination at823 K in air for 5 h ..... Fig. 1. Procedure for the hydrothermal restructuring method
3. RESULTS AND DISCUSSION The yield of Si-MCM-41 was calculated by the weight of calcined sample divided by the amount of SiO2 in the reaction mixture. As the restructuring procedure was repeatedly carried out, the yield of Si-MCM-41 was increased. In case of the usual hydrothermal synthesis, the product yield was about 65 %. The unreacted silica could be actually observed in the filtration solution. In case of the restructured samples, however, the yield of product reached the level of above 90 %. Such a high yield is attributed to the forced pH control which brings about a shift in the reaction equilibrium. It is well recognized that Si-MCM-41 is synthesized in basic medium. In this study, the usual synthesis procedure was carried out under basic condition with a pH value of about 11 [1,4]. The pH of the mother liquor, however, was adjusted to -8 by adding strong acidic solution. When the pH is-8, the solid product disappeared from the reaction mixture and the reaction gel became sticky. This phenomenon caused by the change in pH was similarly observed in the sol-gel process. This viscous solution was not maintained long and turned soft. This indicates that the forced pH control brought about a shift in the reaction equilibrium and promoted the progress of Si-MCM-41 synthesis reaction. XRD patterns of the Si-MCM-41 samples synthesized in the present work are presented in Fig. 2. The patterns for all Si-MCM-41 samples consist of three distinguishable peaks, which can be indexed to different (hkl) reflections of a hexagonal structure [1]. The XRD patterns in parts (c) and (d) of Fig. 2 consist of one very intense line, three weak lines, and one very
104 weak line, which can be indexed to (100), (110), (200), (210) and (300) diffraction lines, respectively, and these represent the characteristics of the hexagonal structure of MCM-41. Figure 2 (a) shows the XRD lines for the Si-MCM-41 samples which were obtained after heating the initial reactant gel mixture in an autoclave at 383 K for 24 h. Here one can clearly observe a strong XRD line broadening and lattice contraction after calcination. These changes are similar with those reported previously by other research groups [6]. In general, the XRD patterns of mesoporous materials shift to the region of higher angle and concurrently the value of d-spacing of mesoporous materials decreases after calcination. This phenomenon is caused by desorption of water, condensation of silica, and loss of structural uniformity. However, the lattice contraction and peak broadening in the samples synthesized by applying the restructuring method were negligible or did not occur at all. The presence of a (300) diffraction line for restructured Si-MCM-41 samples indicates that the high structural uniformity was maintained after calcination. Therefore, it is evident that the restructured SiMCM-41 sample has a high structural stability and the silica species would be completely condensed during the course of restructuring.
(a)
(b)
A~
~ 2
/
._~
calcination
4
6
8
10
2
4
2
4
2O
(c)
6
8
6
8
2O
10
(d)
% cr
#. 2
4
6
20
8
10
20
Fig. 2. XRD patterns of Si-MCM-41 samples: (a) Si-MCM-41 before applying the restructuring procedure; (b) Si-MCM-41 after applying the restructuring procedure once; (c) Si-MCM-41 after applying the restructuring procedure twice; (d) Si-MCM-41 after applying the restructuring procedure three times 9 The as-synthesized samples were washed with distilled water and dried in oven at 373 K, and the calcination was performed in air at 823 K.
105 Figure 3 shows the pore size distributions for the mesoporous samples obtained by the nitrogen adsorption isotherm at liquid nitrogen temperature using the Barrett-Joyner-Halenda (BJH) analysis [1,2,4]. Type IV isotherm, typical of mesoporous materials, is observed and as the relative pressure increases (P/P0>0.25), each isotherm exhibits a sharp inflection, characteristic of capillary condensation within the mesoporous [ 1]. This feature indicates that both samples possess a good structural ordering and a narrow pore size distribution, and also that there has been neither structural nor phase change during restructuring. Furthermore, it is noticed that the restructuring treatment results in a shift in the pore size distribution to the region of lower pore size.
(a)
./'
600
~0
~ 500 400
o 200
ni)i null ,
0.0
"U--n__l__l--l--l--I--l--l--l--I i
0.2
,
i
0.4
Relative
(b)
,
Pressure
i
,
0.6
i
0.8
i
i
i
,
1.0
i ,I
100
(P/Po)
Pore diameter (,h)
600
~
~o 5o0
.~
~
p ~ - i
9
9
I
ii
400
300
i
200
lO0
~n-i-n- 9149
o , 0.o
i
0.2
,
l
i
0.4 Relative
I
i
0.6 Pressure
(P/Po)
i
0.8
,
i
i
1.0
10
,
,
1
,
,
i
| il
,
100 Pore
diameter
i
i
,
,
, ,
(A)
Fig. 3. Nitrogen sorption isotherms and pore size distributions of calcined Si-MCM-41 samples" (a) Si-MCM-41 before applying the restructuring procedure, (b) Si-MCM-41 after applying the restructuring procedure three times. The results of TEM imaging of Si-MCM-41 are shown in Fig. 4. Part (a) shows the image taken in the direction perpendicular to the pores and part (b) the image of viewing down the pore axis. The images along these directions have often been used to identify the hexagonal MCM-41 type phases. These images of Si-MCM-41 revealed a highly mesoporous structure consisting of cylindrical pores arranged on a hexagonal lattice.
106 (a)
(b)
Fig. 4. TEM images of the calcined sample after applying the restructuring procedure three times. The view directions are along (a) the (100) direction and (b) the pore axis. Table 1 presents the structural data of Si-MCM-41 samples. The surface areas of both samples are larger than 800 m2/g, being typical of MCM-41 materials. As given in Table 1, the interplanar spacing dl00 for the calcined parent sample, which did not undergo any restructuring procedure, is 33.82 A and this value ig typical for MCM-41 silicates synthesized using cetyltrimethylammonium bromide as a templating surfactant [ 1, 2]. For the restructured sample which is synthesized with the same reactant composition, the increase in d-spacing was larger than that for the sample synthesized by the usual hydrothermal method. In the present work, the value of 2 0 was reduced by 0.47 while the d-spacing was increased by 7.43 A. This result is related to the shift of XRD patterns to the left-hand side. Of particular relevance to the present study is the pore wall thickness of the Si-MCM-41 materials; the average pore diameter and the pore wall thickness calculated by using the BJH method are given in Table 1. In case of the restructured sample, desorption and adsorption average pore size was decreased whereas the wall thickness was increased. Concerning the textural properties, the pore diameter increases in general if the XRD line shifts to the left. When surfactants of different alkyl chain lengths and different micelle swelling agents are used for the synthesis of Si-MCM-41, the samples synthesized would have different pore diameters [1,2]. As the pore size increases, the (100) reflection shifts to the left (i.e., the value of 2 0 decreases) and the d-spacing increases. The textural data from XRD register an increase after the hydrothermal restructuring treatment. The nitrogen sorption data, however, shows that the pore size was decreased after the restructuring treatment. This was certainly caused by the forced pH control and the subsequent hydrothermal treatment. During the step of pH control, the unreacted silica species in mother liquid are dissolved and during the reheating process, these dissolved silica species take part in the MCM-41 synthesis reaction again.
107 Table 1. Structural properties of Si-MCM-41. Si-MCM-41: usual systhesis method
Si-MCM-41: restructuring procedure three times
Surface area (m2/g)
955
878
20
2.61
2.14
d- value (dl00;A)
33.82
41.25
Unit cell parameter (a0A)
39.05
47.63
BJHdes average pore diameter (A)
32.2
29.8
BJHdes wall thickness(A)
6.85
17.83
BJHads average pore diameter (A) BJHads wall thickness (,~)
33.9
33.6
5.15
14.03
ao = the lattice parameter, from the XRD data using the formula ao = 2dlo o~f3, wall thickness = ao - pore diameter
4. CONCLUSIONS The Si-MCM-41 prepared by the usual hydrothermal synthesis method has been treated by the restructuring method, which consists of the forced pH control step and the subsequent rehydrothermal treatment step. It is found that the restructuring treatment developed in this study can substantially improve not only the yield but also the quality of Si-MCM-41. Indeed, the XRD patterns and the nitrogen sorption data of the treated samples present textural properties different from those of the parent sample. The lattice contraction and peak broadening was negligible or disappeared after calcination. The values of both d-spacing and unit cell parameter are increased and the pore size is decreased. These results were indirect evidence for the effectiveness of hydrothermal restructuring method. The hydrothermal restructuring method gives rise to an improvement in textural properties of mesoporous materials, which is achieved by the condensation of silica species within the pore wall, leading to an increase in the pore wall thickness. In the rehydrothermal procedure, it is evident that the time for the hydrothermal crystallization is extended and the pore. wall is strengthened into a thicker condensed silica frame as a result of the increase in the amount of dissolved silica species during the pH control step. In brief, the forced pH control brings about a shift in the equilibrium of Si-MCM-41 synthesis reaction through the additional dissolution of unreacted silica species. On the other hand, the reheating process promotes the condensation of silica. Therefore, it is obvious that the two steps in the restructuring procedure have a synergistic effect for the increase in the wall thickness.
108 ACKNOWLEDGMENT
This work was supported by Grant No. 2000-1-30700-002-3 from the Basic Research Program of the Korea Science & Engineering Foundation and also partially by the Brain Korea 21 Program of the Ministry of Education.
REFERENCES 1. C. T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359, (i997) 710., J. S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T-W Chu, D. H. Olsen, E. W. Sheppard, S. B. McCullen and J. L. Schlenker, J. Am. Chem. Soc., 114, (1992) 10834., C. T. Kresge, M. E. Leonowicz, W. J. Roth and J. C. Vartuli (Mobil Oil Corp.), U.S. Patent 5098684, (1992). 2. J. S. Beck, U.S. Patent 5057296, (1991)., N. Ulagappan and C. N. R. Rao, J. Chem. Soc. Chem. Commun. (1996) 2759. 3. N. Ulagappan and C. N. R. Rao, J. Ame. Chem. Soc., 116, (1996) 10785., R. Burch, N, Cruise, D. Gleeson and S. C. Tsang, J. Chem. Soc. Chem. Commun., (1996) 951., T. M. Abdel-Fattah and T. J. Pinnavaia, J. Chem. Soc. Chem. Commun., (1996) 665., J. Chui, Y. Yue, Y. Sun, W. Dong and Z. Gao, Stud. Surf. Sci. Catal., Vol. 105, (1997) 69., U. Junges, W. Jacobs, I. Voigt-Martin, B. Krutzsch and E Schuth, J. Chem. Soc. Chem. Commun., (1995) 2283., K. R. Kloestra and H. Van Bekkum Stud. Surf. Sci. Catal., Vol. 105, (1997) 431. 4. J. S. Beck, J.C. Vartuli, G. J. Kennedy, C.T. Kresge, W. J. Roth and S. E. Schramm, Chem. Mater., 6, (1994) 1816., A. Monnier, E Schuth, Q. Huo, D. Kumar, D. Kumar, D. Margolese, R. S. Maxwell, G. D. Stucky, M. Krishnamurty, E Petroff, A. Firouzi, M. Janicke and B. E Chmelka, Science, 261, (1993) 1299., G. D. Stucky, A. Monnier, E Schuth, Q. Huo, D. Margolese, D. Kumar, M. Krishamurty, E Petroff, A. Firouzi, M. Janicke and B. F. Chmeka, Mol. Cryst. Liq. Cryst., 240, (1994) 187., A. Firouzi, F. Atef, A. G. Oertli, G. D. Stucky and B. F. Chmelka, J. Am. Chem. Soc., 119, (1997) 3596. 5. N. Coustel, F. D. Renzo and F. Fajula, J. Chem. Soc. Chem. Commun. (1994) 967., D. Khushalani, A. Kuperman, G. A. Ozin, K.Tanaka, J. Garces, M. M. Olken and N. Coombs, AdV. Mater. 7, (1995) 842., A. Sayari, P. Liu, M. Kruk and M. Jaroniec, M. Chem. Mater. 9, (1997) 2499. 6. C. Y. Chen. S. L. Burkett, H.-X. Li and M. E. Davis, Microporous Mater., 2, (1993) 27.
Studies in Surface Science and Catalysis 141 A. Sayariand M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rightsreserved.
109
Synthesis o f highly ordered mesoporous compounds with control o f m o r p h o l o g y using a non-ioni~z surfactant as template A. L6onard #, J.L. Blin and B.-L. Su* Laboratoire de Chimie des Mat6riaux Inorganiques, ISIS, The University of Namur, 61, rue de Bruxelles, B-5000 Namur, Belgium phone : +32-81-72-45-31, Fax: +32-81-72-54-14, e-mail :
[email protected] Highly ordered hexagonal mesostructures (CMI-1 compounds) can be obtained under mild acidic conditions by working at low concentrations of non-ionic decaoxyethylene cetyl ether [C16(EO)i0]. The present work shows that it is possible to gain control at the nanometer scale over the packing symmetry of the channels, as well as at the micrometer level over the morphology of the particles by varying the surfactant / silica molar ratio and the hydrothermal treatment conditions. Very high loadings of silica precursors typically afford highly ordered hexagonal CMI-1 compounds whereas an increase of the surfactant / silica molar ratio results in materials with a more disordered channel array. In a parallel way, very low molar ratios of surfactant / silica lead to ropes, gyroids and toroids whereas spheres are the most stable shape with the lower quantities of silica. From this point, it appears thus that not only the structure but also the morphologies encountered for MCM-41 type mesoporous silica can be reproduced with a non-ionic templating agent. 1. INTRODUCTION A more environmental-friendly way to prepare large-pore mesoporous materials consists in using polyoxyethylene alkyl ether surfactants as templates because of their lower toxicity and good biodegradability [ 1-6] with respect to their ionic analogues like for example cetyltrimethylammonium bromide, the template generally used in the preparation of MCM-41 [7,8]. Besides, it appears that the recovery of the template is easier and so a further reutilization could be envisaged. Until short ago, the use of these surfactants afforded only disordered wormhole-like structures unless working in very strong acidic media [2] or adding transition metallic cations to the micellar solution [9]. Another way to proceed was to remove the methanol released from the hydrolysis of TMOS by using a rotary evaporator like proposed by Attard et al.[10]. We however recently showed that it was possible to obtain directly highly ordered hexagonal structures of channels (CMI-1 compounds) under mild acidic conditions by working at low concentrations of decaoxyethylene cetyl ether [Cl6(EO)10] [11]. These materials possess very uniformly-sized openings, specific surface areas exceeding 900 mVg and consist of spheres with 1-2 ~tm diameter. A LCT-type cooperative mechanism was proposed to explain the formation of these molecular sieves. It is important to control the structure of the materials. Indeed, if they are to be applied in catalysis, the 3-dimensional structure of MSU is most appropriate whereas the # :FRIA fellow *: Corresponding author
110 production of low-branched polyethylene fibres [12] or the fabrication of semi-conducting wires [13] would require a regular array of long straight channels. Besides this, the morphology turns out to be crucial also. Indeed, spherical particles are the most suitable in chromatographic applications [14]. This work shows that it is possible to gain control over these two aforementioned factors by adjusting the Cl6(EO)10 / silica molar ratio and the hydrothermal treatment conditions. Different characterization techniques (SEM, TEM, XRD and nitrogen adsorption-desorption analysis) have been used to shed light on the morphological, structural, and textural features of the prepared CMI-1 compounds. 2. EXPERIMENTAL 2.1. Synthesis
A 10 wt.% micellar solution was prepared by dissolving 6.67 g of decaoxyethylene cetyl ether [Cl6(EO)10, Brij 56 | in 60 ml water. Sulfuric acid was then added to decrease pH to a value of 2. After homogenization at 70~ TMOS was added dropwise, the quantity depending on the desired surfactant / silica molar ratio (from 0.25 to 3.50). After further stirring during 1 hour, the synthesis gel was poured in teflon-lined cartridges sealed in stainless steel autoclaves. Hydrothermal treatment was performed at 40, 60 and 80~ during 3, 2 and 1 days respectively. The recovered gel was then extracted using a Soxhlet apparatus, dried under vacuum at ca. 60~ and calcined at 550~ under nitrogen and oxygen. 60 ml bidistilled (
water
~
6.67 g C16(EO)lo, [ (Bri~6| y
H2804
Micellar solution (pH 2, 70~ Gel Hydrothermal treatment at 40, 60 and 80~ during 3, 2 and 1 day(s) I
surfactant / TMOS molar ratio = R = 0.25-3.50
Ethanol extraction Drying[ Synthesis scheme of Calcination at 550~
I=:~1 Powders [
orderedcMi.1 materialsmeS~176176
2.2. Characterization
Information about structure was obtained by X-ray diffraction measurements with a Siemens D-5000 diffractometer and transmission electron microscopy was performed on a Philips Techna'f microscope with an acceleration voltage of 100kV. The powdery samples were embedded in an epoxy resin and sectioned with an ultramicrotome before being
111 deposited on carbon, coated copper grids. The textural properties of our compounds were assessed by nitrogen adsorption-desorption measurements. Analysis took place over a wide range of relative pressures on a Micromeritics ASAP 2010 or Tristar 3000. The pore diameter and the pore size distribution were determined by the BJH method [15] although it is well known that this method gives underestimated pore size values and that some new interesting methods have been developed recently by Jaroniec et al. [ 16]. However, this will not affect our systematic comparison as the same method was used for all of the experimental results. Morphological features have been investigated with the use of a Philips XL-20 scanning electron microscope. For conductivity purposes and in order to enhance the yield of secondary electrons, powders were first covered by a thin layer of gold by metallization. 3. RESULTS AND DISCUSSION 3.1. Information about structure 3.1.1. Determination of the arrangement by XRD
Only the lowest surfactant / silica molar ratios (R) have been investigated by XRD measurements because of the very small quantity of materials obtained as the molar ratio increases. As the walls of the mesoporous compounds are amorphous, the quality of the materials will be reflected by the regular repetition of the pore to pore distance which is characterized by a very strong feature at low angles. If the packing symmetry of the channels is regular in space, secondary reflections will appear on the diffractograms. For example, in the case of MCM-41, besides the sharp 100 peak, additional 110, 200, 210,...features will be visible on the diffractogram. In that case, it is possible to determine the cell parameter a0 = 2d~00/3 ~r2,which represents the sum of the pore diameter and the wall thickness. 1 day at 80~
2 days at 60~
3 days at 40~
'II- 5.3 nm
4 5.7 nm
5.7 nm
V••'l •-
I
R = 1.50
//1~0 7 9 nm
t~ 3.1nm
,,
~-" 5.3 nm
.==
~-5.4 nm
~1-- 5.5 nm
.t=t
R = 0.50
3.2nm
3.8nm ',~ l~2.7nm ~ _
_
2
_
/ 3.1nm
. . . . ,
4
.
.
.
6
.
20 (o)
.
-
8
10 2
.
.
.
.
20 (o)
.
.
8
lo
2
.
.
4
.
:
6
20 (o)
.
:
8
.
10
Figure 1" XRD patterns of samples prepared at different hydrothermal treatment conditions and with 2 surfactant / silica molar ratios (R) The multi-peak pattern characteristic of hexagonal materials can be clearly evidenced for the sample prepared at 80~ with a surfactant / silica molar ratio of 0.50. Using the Bragg law to calculate the d-spacings, the unit cell parameter can be determined to be equal to 6.2 nm. Increasing the surfactant / silica molar ratio does not influence the aspect of the diffractograms. However, if hydrothermal treatment is performed at 60~ the secondary
112 reflections are less well resolved and their intensity drops with the amount of added silica. If R exceeds 1.00, no secondary peaks can be evidenced any more, suggesting the appearance of a disordered network like MSU materials. At 40~ the 110 and 200 reflections drop in intensity with increasing R suggesting the appearance of a less ordered channel array. The hydrothermal treatment conditions as well as the surfactant / silica molar ratio (R) do not seem to have an effect on the unit cell parameter which remains between 6.1 and 6.8 nm. However, lower amounts of added silica have a strong influence on the structure of the samples. As R augments, the regular structure is progressively lost and materials are more likely to belong to the family of MSU rather than CMI-1. 3.1.2. TEM observations
Figure 2 shows the TEM pictures of the compounds that were obtained under different conditions of hydrothermal treatment and at molar ratios ( R ) o f 0.50 and 1.50. The molar ratios that were studied ranged from 0.25 to 3.50. From a general point of view, it appears that the compounds are well ordered if the R value remains below 1.50. The hexagonal "honeycomb-like" arrangement of the channels characteristic of CMI-1 is clearly visible on the TEM micro graphs . The inserted Fourier Transforms show hexagonally dispersed spots, confirming the hexagonal packing symmetry that was suggested from XRD measurements. However, if the surfactant / silica molar ratio increases beyond this value, the regular empilement is progressively lost, more rapidly at 60 than at 80 or 40~ Even if arranged channels can still be found on the grid, these zones become much more sparse when the amount of added silica decreases. This phenomenon is the most amplified at 60~ It appears thus that there is coexistence between regular CMi~-1 material and disordered MSU-type for the higher molar ratios. I day at 80~
2 days at 60~
3 days at 40~
R = 1.50
R = 0.50
Figure 2" TEM pictures and inserted Fast Fourier Transforms of samples prepared at different hydrothermal treatment conditions and with 2 surfactant / silica molar ratios (R) In all cases, the compounds evolve towards wormhole-like disordered structures as the added silica becomes less. Interestingly, the materials are not as well ordered at 60 than at 80 or 40~ whatever the value of R is, according to the results obtained by XRD and TEM. From all of these observations, it can be postulated that the amount of added inorganics plays a key role in the organization of our materials. Indeed, for low surfactant / silica molar ratios, i.e. for high contents of tetramethoxysilane, all the isolated micelles are covered by a shell of inorganic material and these supramolecular entities can self-assemble in
113 order to form the regular structure through a cooperative mechanism in agreement with our previous results [11 ]. The higher the ratio or the lower the silica content, the less regular the organization. One could imagine that there are not enough silica oligomers present in solution to perform a complete condensation of all these silica rods. In this case, the regular hexagonal packing symmetry, though still present at some places, does not prevail over the whole extend of the material. Places of disordered wormhole-like materials are then formed when the channels move one from each other in order to form a continuous silica framework. The first regular organization of CMI-1 materials was reported for samples prepared at a surfactant / silica molar ratio (R) of 1.50. Above results show that a very regular array of channels can also be obtained at a R value as low as 0.50 and so, the higher concentration of methanol released in this case (1.30 mol/1 compared to 0.44 mol/1 for the original preparation of CMI-1) seems not to disturb the formation of the regular structure. (Since it was previously reported that the threefold larger amount of released methanol could play a role of liquid crystal breaker [ 1,10]) Present observations strongly confirm our previous proposition that it is the interaction between the hydrolyzed silicic species and the hydrophilic heads of the surfactant that will determine the final structural geometry of the pores.
3.2. Nitrogen adsorption-desorption analysis Figure 3 depicts the isotherms and the pore size distributions (inserts) of materials obtained for R values of 2.50 and 0.50 for different hydrothermal treatment conditions. At 80~ all the isotherms are type IV, characteristic of mesoporous compounds. The capillary condensation step locates at around p/p0 = 0.54, whatever the molar ratio R is, suggesting constant pore diameters. This step however seems to be more steep for the lower values of R suggesting a better homogeneity in the pore sizes. This is verified on the pore size distributions which are very narrow and centered at 4.2 + 0.4 nm. For all of the amounts of added silica, the specific surface areas of mesoporous compounds are very high (Table 1). Table 1 : Textural and structural features of the samples as a function of surfactant / silica molar ratio (R) and hydrothermal conditions. Hydrothermal treatment
SBET(m2/g) 0.50 2.50 0.50 2.50
920 830 1182 2 days at 60~ 616 o15o 1096 3 days at 40~ [ 2.50 913 n.d. "no data, - "not observed, * 9from XRD data. 1 day at 80~
. ,
Pore diameter (nm) 4.1 4.3 3.4 3.8 3.8
Cell parameter ao (nm)* 6.2 n.d. 6.4 n.d. 6.1 n.d.
If treatment is performed at 60~ isotherms are type IV only for the molar ratios below 1.5 and get a shape located between type I and IV for the higher ratios, characteristic of supermicroporous compounds. If the surfactant / silica molar ratio varies from 1.50 to 3.50, the maximum of the pore size distributions passes from 3.4 to a value less than 2.0 nm (Fig.3). This shift toward supermicroporosity could be explained by a rearrangement of the micellar solution. Indeed, polymerization at 60~ is not as extended as at 80~ and so, to maximize interactions between silica species, a rearrangement could occur in the synthesis gel forming smaller micelles leading to a continuous silica network with shrinked openings. This phenomenon is accompanied by a loss of the regular ordering of the channels. As already
114 discussed in literature, the characteristics of the final framework result from an interplay between inorganic and organic species present in solution [1,11]. Evolution at 40~ is a bit more particular in the sense that secondary mesoporosity appears for the molar ratios that exceed 0.50. Indeed, isotherms are type IV for the high loadings of added silica whereas the adsorbed volume at high relative pressures strongly I day at 80~
800 o.o~ oo
R = 2.50 ~ 600 ~400
40011
2 days at 60~
3 days at 40~
0.03
1 oo!
3o0 o0
1000
0o,
200 800
600
800
200 /-
200 1/ "
200.
0.0 0.2 0.4 0.6 0.8 1.0
Relative pressure p/po
0.0 0.2 0.4 0.6
0.8 1.0
Relative pressure P/Po
0.0 0.2 0.4 0.6 0.8 1.0
Relative pressure p/Po
Figure 3 :Nitrogen adsorption isotherms and inserted pore size distributions of samples prepared at different treatment conditions for 2 surfactant / silica molar ratios (R). increases when there are less silica species in solution. The higher the R value, the more secondary mesoporosity appears. The extend of polymerization increases with temperature. For example, the masses of powdery materials obtained at 40, 60 and 80~ for R being equal to 0.25 are 1.30, 1.82 and 2.00 g respectively. For the higher surfactant / silica molar ratios at 40~ a rearrangement of the micellar solution like observed at 60~ would not be the best way to obtain maximum polymerization and instead of this, holes would remain in the structure. This hypothesis could explain the appearance of secondary mesoporosity and the constant pore diameters at 40~ Indeed, the maximum of the pore size distributions remains practically constant (3.5-3.8 nm). Nevertheless, rearrangements of the channels are likely to occur leading to more disordered wormhole-like structures. This explains the less good organization for the higher surfactant / silica molar ratios.
3.3. Morphological features The morphologies of the samples prepared at different surfactant / silica molar ratios and at variable conditions of hydrothermal treatment are shown in Figure 4. At 80~ if the loading of added silica is very high (R = 0.25), the majority of the sample is made of hexagonal-shaped ropes with a length of several microns. For a R value of 0.50, the toroids and gyroids prevail and when the surfactant / silica molar ratio is equal to 1.00, we can observe a mixture of toroids and spheres. Beyond this value, only spheres are present. There is thus a clear evolution from ropes to gyroids and finally towards spheres as the surfactant / silica molar ratio increases. These peculiar morphologies have already been encountered by Ozin and his coworkers who used an ionic templating agent and TEOS as inorganic source [17,18]. The syntheses were carried out at room temperature or 80~ and the preparations were done in a
115 quiescent state as agitation led to the same morphologies, but with more broken forms. They proposed that a silicate liquid crystal embryo with a hexagonal cross-section evolves into several morphologies with degrees of curvature that depend on the initial reaction conditions. 1 day at 80~
2 days at 60~
3 days a t 4 0 o c
R = 2.00
R = 0.50
R = 0.25
Figure 4 : SEM pictures of samples prepared at 80, 60 and 40~ and with surfactant / silica molar ratios of 0.25, 0.50 and 2.00. A lower acidity or an increase in temperature favour the preparation of spheres rather than gyroids [19,20]. They pointed out that higher acidic quiescent conditions afford rapid growth and polymerization of a silicate liquid crystal seed where polymerization induces local rigidification effects that dictate the curvature. In this case, there is a smooth and continuous deposition of silicate-micellar species on specific regions of the liquid crystal seed, which results in the formation of gyroids. When pH value is increased or when the syntheses are performed at 80~ there is a slower global silicification and the curvature results from surface tension forces. The slower polymerization at lower acidity makes thus surface tension the overriding shape-controlling factor and spheres minimize surface area and surface free energy. In our present study, pH value remained constant throughout all of the syntheses, but only the surfactant / silica molar ratio as well as the hydrothermal treatment conditions were changed. However, for the lower molar ratios, there are a lot of silica oligomers present in solution. So, we could deduce that, the more silica present in solution, the more polymerization will induce local rigidification effects, resulting in the specific local deposition of silica species affording ropes or gyroids. When the amount of inorganics present in solution is progressively decreased, i.e. for the higher molar ratios, the growth process will not be controlled by the polymerization any more. The more preferential mechanism will be the minimization of the surface tension at the surfactant / silica interface and thus the most stable resulting shape is the sphere. A similar evolution is observed at 60~ although the morphologies are not as well defined as at 80~ Spheres are the only morphology that exists at higher values of R. At 40~ the evolution of morphology is a bit more particular. For high loadings of tetramethoxysilane, toroids and ropes can be detected, just like at 60 and 80~ When the ratio is increased beyond 1.00 however, the characteristic morphologies can still be found but
116 have no smooth surfaces any more but rather a more broken appearance. At a ratio of 2.00, the surfaces of the particles become more and more broken and the shapes, though still suggesting the toroidal and gyroidal morphologies, start to be more stochastic. These observations are consistent with the results of the adsorption-desorption measurements. The fact that the particles are not as smooth any more on their surfaces is coherent with the appearance of secondary mesoporosity as the surfactant / silica molar ratio is increased. The more spongy appearance of the samples preiaared at 40~ comes from a less advanced polymerization at lower temperatures and, above all, at higher surfactant / silica molar ratios. 4. CONCLUSION The influence of the amount of added silica on the internal as well as external morphologies of mesoporous compounds has been evidenced. From a general point of view, the packing symmetry of the channels tends towards a wormhole-like one if less silica species are present in solution. A high concentration of TMOS typically leads to "exotic" morphologies already encountered for MCM-41 type materials. Also, hydrothermal treatment conditions have a drastic influence on structure, texture and morphology. ACKNOWLEDGEMENTS
This work has been performed within the framework of PAI/IUAP 4-10. Alexandre L6onard thanks FNRS (Fonds National de la Recherche Scientifique) for a FRIA scholarship. REFERENCES
1. G.S. Attard, J.C. Glyde and C.G. GSltner, Nature, 378 (1995) 366. 2. D. Zhao, Q. Huo, J. Feng, B.F. Chmelka and G.D. Stucky, Jr. Am. Chem. Soc., 120 (1998) 6024. 3. E. Prouzet and T.J. Pinnavaia, Angew.Chem.Int. Ed. Engl., 36(5) (1997) 516. 4. E. Prouzet, F. Cot, G. Nabias, A. Larbot, P. Kooyman and T.J. Pinnavaia, Chem., Mater., 11 (1999) 1498-1503. 5. S.A. Bagshaw and T.J. Pinnavaia, Angew. Chem.Int. Ed. Engl., 35(10) (1996) 1102. 6. P.T. Tanev and T.J. Pinnavaia, Science, 267 (1995) 865. 7. J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T-W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins and J.L. Schenker, J. Am. Chem. Soc., 114 (1992) 10834. 8. C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli and J.S. Beck, Nature, 359 (1992) 710. 9. W. Zhang, B. Glomski, T.R. Pauly and T.J. Pinnavaia, Chem.Commun.,(1999) 1803. 10. N.R.B. Coleman and G.S. Attard, Microp. and Mesoporous Mater., 44-45 (2001) 73-80. 11. J.L. Blin, A. L6onard and B.L. Su, Chem. Mater. 13(10) (2001) 3542. 12. K. Kageyama, J.I. Tamazawa and T. Aida, Science, 285 (1999), 2113. 13. C.G. Wu and T. Bein, Chem. Mater., 6 (1994) 1109. 14. C. Boissi6re, A. van der Lee, A. E1 Mansouri, A. Larbot and E. Prouzet, Chem. Commun., (1999) 2047. 15. E.P. Barret, L.G. Joyner and P.P. Halenda, J. Am. Chem. Soc., 73 (1951) 373. 16. M. Jaroniec, M. Kruk and A. Sayari, Stud. Surf Sci. Catal., 129 (2000) 587. 17. H. Yang, N. Coombs and G.A. Ozin, Nature 386 (1997) 692. 18. G.A. Ozin, H. Yang, I. Sokolov and N. Coombs, Adv. Mater. 9(8) (1997) 662. 19. G.A. Ozin, C.T. Kresge and H. Yang, Stud. Surf. Sci. Catal. 117 (1998) 119. 20. H. Yang, G. Vovk, N. Coombs, I. Sokolov and G.A. Ozin, Jr. Mater. Chem., 8(3) (1998) 743.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
117
Towards a better understanding on the mechanism o f mesoporous formation via an assembly o f Cn(EO)m and T M O S J.L. Blin, A. L6onard #, G. Herrier #, G. Philippin and B.-L. Su* Laboratoire de Chimie des Mat6riaux Inorganiques, ISIS, The University of Namur (FUNDP), 61, rue de Bruxelles, B-5000 Namur, Belgium The present work deals with a systematic study of mesoporous materials synthesis. A series of polyoxyethylene alkyl ether surfactants such as Cl3(EO)n (n = 6, 12, 18), C16(EO)10, CI8(EO)I0 have been used. It is revealed that the surfactant conformation changed with the heating temperature. Indeed, at higher temperatures, a more extended molecular conformation can be obtained, which leads to materials with larger pore sizes. We have also shown that the interaction between template and silica disturbs the hexagonal array of micelles in solution leading to the formation of DWM-1 or DWM-2 compounds for concentrated micellar solution. We have also correlated the structural characteristics of the recovered mesoporous molecular sieves with the VH/VL ratio of the template.
1. INTRODUCTION Owing to their large internal surface area, open three dimensional structure, and adjustable chemical properties, microporous materials such as zeolites have widespreadly been used in chemical and petrochemical industry. However, because of their limited pore sizes, the treatment of more bulky molecules requires new solids able to provide catalysts or adsorbents with larger openings. The synthesis efforts have culminated in 1992 when Mobil researchers reported the preparation of several mesoporous silicates with unique pore structures [1, 2]. Tunable openings have been obtained by using cationic surfactants with variable hydrocarbon tail lengths as templating agents and by adding some auxiliaries like, for instance, organic swelling molecules. The synthesis of mesoporous molecular sieves consists of the condensation and polymerization of an inorganic precursor around the micelles of surfactant. Until now, a large series of cationic, anionic, gemini and neutral surfactants have been used in the synthesis of ordered mesoporous silicas or non-silicas and materials labeled MCM, HMS [3], TUD [4], SBA [5], MSU [6] and CMI [7] have been obtained. The synthesis of the last ones is achieved through a neutral N~ ~pathway, in which hydrogen bondings are responsible for the cohesiveness between the non-ionic recoverable and biodegradable surfactant (N~ and the inorganic precursor (I~ The first syntheses of mesoporous molecular sieves achieved by using such non-ionic polyoxyethylene alkyl ether [Cm(EO),] surfactants were reported by Attard et al. [8] with octaethylene glycol monododecyl ether [CI2(EOs)] and octaethylene glycol monohexadecyl ether [Cm6(EOs)]. However, the regular mesoporous obtained by this group [9] was only owing to the gentle removal of the large amount of methanol released from the hydrolysis of TMOS used as silica precursor. Indeed they found # : FRIA Fellow * : Corresponding author
118 that methanol played a role of liquid crystal breaker destroying the hexagonal H1 phase formed by the surfactant molecules in aqueous solution. Nevertheless, recently, via a new pathway [(N~ ~ which involves the formation of hydrogen bonds between a cationic metal (M "+= Li+, Co 2+, Mn2+, and Zn2+) complex form of a non-ionic polyoxyethylene surfactant (N ~ and the neutral inorganic precursor (I~ Pinnavaia et a/. [ 10] have successfully oriented the structure of the final silica compounds working at a very low concentration of around 1.8 wt.% in neutral media. Cubic SBA-11 and hexagonal SBA-!2 were obtained using CI6(EO)10 and Cls(EO)10 respectively at a weight percentage of 4-6, the syntheses being performed at room temperature in strong acidic media (pH << 1) [6]. Recently, it was reported that disordered wormhole-like mesoporous silicas, zirconium oxides [11] and titanium oxides [ 12] could be synthesized with neutral surfactants and two types of disordered wormhole-like mesostructures (DWM-1 and DWM-2) were distinguished. DWM-1 type materials are quite similar to MSU, while DWM-2 exhibit relative inhomogeneity in their pore sizes, explaining the absence of XRD reflections. However, behind this important and encouraging progress and the strong attraction of new materials synthesis, less knowledge has been acquired on the synthesis mechanism, despite the lot of results published and available in literature. Moreover, there are important divergences in scientific findings from different authors. These disparities mainly result from the different, even though slightly, synthesis conditions and have been objet of a dispute that is far from being settled. The present work deals with a systematic study of silica mesoporous materials synthesis. A series of polyoxyethylene alkyl ether surfactants such as C13(EO)n (n = 6, 12, 18), CI6(EO)I0, C18(EO)~0 have been used. The present research is expected to enlarge the amount of available informations on the synthesis mechanisms of mesoporous materials. 2. EXPERIMENTAL 2.1. Synthesis A micellar solution with a weight percentage of Cm(EO)n varying from 5 to 60 was prepared by dissolving the surfactant at a temperature below the cloud point value in an aqueous solution during 3 hours. The pH value of the micellar solution was then adjusted with H2804 to 2.0. The obtained medium was stirred for three hours at this temperature before adding drop by drop the silica source 9tetramethoxysilane (TMOS). The surfactant / silicium molar ratio is fixed to 1.5. The obtained gel was sealed in Teflon cartridges enclosed in stainless steel autoclaves and heated. The final products were recovered after ethanol extraction with a soxhlet apparatus during 30 hours and calcination under nitrogen and then air atmosphere at 550~ for 18 hours in order to remove all the surfactant and impurities.
2.2. Characterization The XRD patterns were obtained with a Siemens D 5000 diffractometer. The transmission electron micrographs were taken using a 100 kV Philips Techna'f microscope. For TEM observations, sample powders were embedded in an epoxy resin and then sectioned on an ultramicrotome. The morphology of the final phases was studied using a Philips XL-20 Scanning Electron Microscope (SEM) with conventional sample preparation and imaging techniques. Nitrogen adsorption- desorption isotherms were obtained at -196 ~ with a volumetric adsorption analyzer ASAP 2010 or TRISTAR 3000 both manufactured by Micromeritics. The samplrs were further degassed under vacuum for several hours before nitrogen adsorption measurements. The pore diameter and the pore size distribution were determined by the BJH method [ 13].
119 3. RESULTS AND DISCUSSION 3.1. Effect of the hydrothermal treatment duration and temperature This study was performed for compounds prepared with 50 wt.% of surfactant. This loading of surfactant corresponds to a region where the hexagonal array of the micelles (HI) is present in solution [14]. 3.1.1 Structure of the prepared compounds. The structural investigations show that the materials obtained with decaoxyethylene cetyl ether [C16(EO)10] and decaoxyethylene oleyl ether [Cls(EO)10] belong to the DWM-1 (or MSU) family. Indeed, only one peak is observed by XRD (Fig. l a). This reflection line is related to the sum of the pore diameter and the wall thickness. The TEM pictures confirm the wormhole structure of the channels (Fig. l b). In contrast, the use of polyoxyethylene (6) tridecyl ether [C~3(EO)6]affords materials that, in spite of a relatively homogeneous pore size distribution, do not show any peak on their XRD patterns. These compounds belong to the family of DWM-2. In any case, when working with a weight percentage located in the H1 domain, we could expect that the recovered materials should have the hexagonal array of their channels, similar to the "micellar mould". However, the XRD and TEM results show that the compounds belong to either DWM-1 or DWM-2 families. This led us to conclude that the addition of the silica source disturbs the micellar array formed in solution. The mechanism represented in Figure 2 has been proposed to explain the formation of materials when Cl6(EO)10 and Cls(EO)10 are used as template. When the TMOS is added to the aqueous solution of micelles having a hexagonal structure (HI), hydrogen bonding type interactions between the oxygen atoms of the ethoxy head groups of the surfactant and hydrogen atoms of the silica source occur. Then, the polymerization of silica disturbs the regular H1 micellar array and the channels slightly move in order to minimize steric and electrostatic energies. Thus, the regular organization of the preformed micelles is lost and the obtained materials will be disordered. Only one broad peak is detected on the XRD pattern, channels with a wormlike structure are observed by TEM and a H2 type hysteresis loop can be noted from nitrogen adsorption, which indicates that the recovered compounds are DWM-1 materials. However, when Cl3(EO)12 and C13(EO)6are used, the interaction between surfactant and silica, as well as the repulsion between hydrophilic headgroups lead to the formation of DWM-2 (See below). Table 1 sums up the different structures obtained with Cm(EO)ntemplates.
Table 1 : Different structures obtained with Cm(EO)n. CMI-1 Surfactant (wt.%)
CMI-3
DWM-1
DWM-2
C16(EO)I0(5-25) CIs(EO)10(< 30) C16(EO)I0(> 25) C13(EO)12(>- 15) C~s(EO)10 (-> 30) C13(EO)6(5-50) Cl3(EO)12 (< 15)
3.1.2 Textural features. The textural characteristics of the materials are summed up in table 2. From these, it is evident that increasing heating temperature favors the formation of large pore mesoporous molecular sieves. Sierra et al. [ 15] have reported the synthesis of mesoporous materials using
120 polyethyleneglycol-4,terocylphenylether with 9-10 ethoxy groups (Triton X100) as surfactant and sodium silicate as silica source. They have concluded that the pore size depends on the polycondensation of the silica, which is increased with temperature, and on the surfactant conformation. These authors explain the expansion of pore size with increasing pH from 2 to more than 8.5 by considering a change in the surfactant conformation and the arrangement of the polyoxyethylene chains on the surface of silica. However, no details have been given on how and in which manner the conformation of surfactant changes. In the present work, the variation of the pore diameter of mesoporous materials with increasing temperature can also be interpreted from the point of view of the change in the surfactant conformation. At low heating temperature, in an aqueous solution of polyoxyethylene alkyl ether, the hydrophilic part of the surfactant exhibits a contracted conformation due to its large number of hydrogen bondings with water molecules (Fig. 3a). Contacts and interaction of the ethoxy oxygens with the silanol groups of the silica are not favored by this conformation. The effective crosssectional area of the hydrophilic headgroup of the surfactant is important. According to Kunieda et al. [ 16], micelles with a high curvature and a small diameter are therefore formed. If the heating temperature is raised, the water molecules bound around ethoxy groups through hydrogen bonds disappear progressively and a more extended conformation is expected (Figure 3b). The curvature of the micelles will thus decrease. This conformation allows more interactions with silica but needs a larger area on the silica walls to be achieved. The consequence is an increase in the pore diameter. _
2
4
6
8
10
12
_
14
20 (o)
Figure 1 9XRD pattern (a) and TEM micrograph (b) of a typical DWM-l-type sample and TEM micrograph (c) of a DWM-2 sample (see Table 1). I ~ phase o f m i c e l l e s i n aqueous solution
Destruction o f the H l p h a s e d u e to 9
interactious at the interface o f s i l i c a , 9 source and P E O , , 99
9
9 1r 4o 9E r
~
.. , ~
9
_o _n
E O~
o
,,
-,,.
Figure 2 9Effect of the addition of silica to the hexagonal array of Cm(EO)nmicelles.
121 Table 2" Variation of the pore diameter (nm) with heating time and temperature Heating time (days) 0.5 1
2 3 4 5 6
60~
80~
100~
60~
4.5 5.5 5.6
5.0 6.5 6.3
6.8 11.7 10.3
1.7 1.7
9.4 6.7 5.8 5.2 4.5 4.8 7.9
-
7.3
9.1
15.6
.
8.2 9.3
8
CIs(EO)I0
C16(EO)I0
C13(EO)6
11
80~
100~
5.2
7.5
4.7 4.0 12.9 9.9 12.1 12.1
8.0 13.4 15.8 17.1 14.6 -
60~
80~
7.0 7.6
5.7 9.1 8.2 10.1
10.6
100~ 8.1 7.8 14.7 13.6 14.4
- : no data
I lip~
I
H,20 ~0 ~C C~ 2 I H2
~CH21
C H 2~ / C H 2 "0 " I
CH
/ C H2 2~0 "
2o
I lipophilic }--- o
Ci2
H,20 I ~0 ~C
I
~ ~o
H,20 18 H " C~ 2
] H2
C H 2~ / C H 2 "0 " I
~ ~o
,~0 ...CH .,,.CH /0 ...CH~. 0/.C H2,C OH cH?H2~o ~C H2~CH2 ~CH 2 2~0 2~CH2 ~CH 2 H2""
Figure 3 9Different conformations ofpolyoxyethylene alkyl ether a" at low temperature, b" at high temperature 3.2 Variation of the weight percentage of template
In the case of decaoxyethylene cetyl and oleyl ether, when the preparation was carried out at surfactant weight percentages that, according to the phase diagram, afford only isolated micelles in solution (10 wt.% of C16(EO)10for instance), the compounds exhibit a multi-peak XRD pattern (Fig. 4). The presence of secondary reflections, in addition to the first sharp peak, is suggestive of a high organization of the channels in our material. Indeed, these reflections can be indexed in a hexagonal system and are related to the 100, 110 and 200 peaks. CMI-I [7] and CMI-3 [17] materials are respectively obtained. The hexagonal arrangement is confirmed by the TEM analysis (Fig. 5b and c). The Fourier transform pictures of TEM images exhibit sixfold symmetry and the measured angles between two bright spots are very close to 60 ~. If the weight percentage of template is increased, the secondary reflections (110 and 200) decrease in intensity and f'mally disappear. This indicates the formation of the disordered structure (Fig. 5a).
122
r~
"'J
30wt.%
60~.%
20wt.%
45wt~%
~
B,I
20( ~) Figure 4 9Variation of the XRD patterns of samples prepared with the weight percentage of CI6(EO)10.
Figure 5" Variation of the TEM micrographs of samples obtained with the weight percentage of C16(EO)10 fl: 50 ; b and c : 10.
Pathway A of Figure 6 is used to explain the molecular sieve formation. It is analogous to that developed by Mobil's scientists [1]. First, isolated micelles of surfactant are formed since the concentration of surfactant in aqueous solution is low. When the silica is added as mentioned above, hydrogen bonding interactions between the oxygen atoms of the ethoxy head group of the surfactant and hydrogen atoms of TMOS appear. To complete polymerization of tetramethoxysilane, these rod-like supramolecular assemblies (templatesilica) have to pack together, which involves a highly ordered arrangement of the channels as it can be seen from the TEM micrographs. This involves a cooperative mechanism, i.e. hydroxyl groups of silica source produced by the hydrolysis reaction interact with hydrophilic chain heads of surfactant molecules and the polymerization of silica species at the interface of rod micelles attracts the rod micelles covered by the silica source together to form a regular arrangement, leading to CMI-n materials. Concerning the polyoxyethylene tridecyl ethers, evolution is quite different. For C~3(EO)12 only one reflection, characteristic of DWM-l-type materials is observed by XRD when the weight percentage of template is decreased, whereas no reflection is detected for C~3(EO)6. Stucky et al. [18] have shown that the molecular packing model used to describe the water-surfactant systems could be extended to mesoporous silicate structures. The surfactant packing parameter g is defined as V/a~ 1r where V is the volume of the molecule, as is the headgroup area and 1r is the critical length of the hydrophobic tail. Small values of g stabilize more curved surfaces such as MCM-41 (1/3 < g < 1/2), while larger values of g stabilize less curvature such as MCM-48 (1/2 < g < 2/3) or lamellar MCM-50 (g = 1). The formed mesostructure can be thus controlled by this parameter. Based on a method proposed by Stucky et al. [19], we have determined the ratio between the volume occupied by the hydrophilie and lypohilic parts of the surfactants (Vn/VL). The values are summarized in Table 3. \
123 Interaction at interface of silica source and PEO
J l
Agglomerates of single rod micelles owing to a cooperative pathway
Single rod micelles in aqueous solution ~ E
Ep
,,W,.EoA~~
"Q, o.-~n
~,., Eo Eo
o
.._ ,,o " , , ; T . e,~,.~ = OH
O11
O.U
EO E6EO EO
~
.~ 0
"
~'~'o
~~
0
l Figure 6 9Effect of the addition of silica to the isolated micelles of Cm(EO)n. In the case of ionic templates and in particular for quatemary ammonium salts CnTMAX (X = C1, Br, OH...) it was reported that if n is located between 6 and 18, the hexagonal MCM-41 structure is formed whereas for n >18 only an amorphous phase is obtained [20]. It was however reported that C22 alkyl chains could lead to MCM-41 if the methyls of the headgroup were replaced by ethyl entities [21]. No micelles are formed if the value of n is less than 6. In the present study we propose that the VH/VL ratio can play a similar role as n. When Cl3(EO)is is used as template the repulsion between the hydrophilic headgroups of the surfactant is more important. Considering the proposed mechanism in Figure 6 (pathway B), surfactant-silica interfaces will be strongly perturbed by these headgroup interactions leading to materials with a disordered MSU-type network of channels. This phenomenon is reflected in the VH/VL values, which are much higher for these two templates compared to C16(EO)10and C18(EO)10 that posses a similar ratio and the same final structures. For the C 1 3 ( E O ) 6 , whatever the weight percentage of template is, neither highly ordered CMI-n nor disordered DWM-1 compounds are obtained. The materials possess a relatively narrow pore size distribution but no peak can be detected on the XRD patterns suggesting thus a degree of structural order even less than DWM, 1-type compounds. Taking into account the ratio ofhydrophilic to hydrophobic volumes, it appears thus that there would be an optimal ratio that could lead to ordered structures. Disordered but homogeneous frameworks would likely be formed beyond this value whereas smaller hydrophilic portions of the template would not afford any structured materials. Additional syntheses implying
124 Table 3 : Contribution of the hydrophilic (Vn) and lypophilic (VL) part of surfactant, obtained structure and weight percental e below which this phase a 1~pears (wt.%).
C13(EO)6
CI6(EO)Io
CI3(EO)12
C13(EO)18
1.23
1.39
2.04
3.04
Obtained structure
Hexagonal
Hexagonal
Wormhole
Wormhole
wt.%
30
25
15
VH/VL
1.04
CI8(EO)I0
a : amorphous, * value not yet determined polyoxyethylene tridecyl ether with headgroups such that the VH/VLratio is in the same range as C16(EO)10 and Cls(EO)10 will be performed in order to verify this hypothesis. 4. CONCLUSION With use of the results gathered during this work, we tried to shed some light on the possible synthesis mechanisms of mesoporous compounds by using non-ionic polyoxyethylene alkyl ethers as surfactant. Whatever the template is, if the weight percentage is located in the range where the hexagonal array is detected on the phase diagram, the addition of TMOS disturbs the arrangement of the micelles in solution. Indeed, when the tetramethoxysilane molecules are added to the aqueous solution of micelles having a hexagonal structure, their interactions with surfactant molecules induce a displacement of the channels and the recovered materials have the DWM characteristics When decreasing the weight percentage of decaoxyethylene cetyl or oleyl ether, well ordered CMI-n materials can be prepared. In this case, isolated micelles are formed in solution and after the addition of silica, to reach a complete polymerization of tetramethoxysilane, the supramolecular template-silica assemblies have to pack together, which evolves toward a highly ordered arrangement of the channels. This is a cooperative effect of interface interactions of hydroxyl groups of silica source-rod micelles and polymerization of silica source covering the outer layer of rod micelles. Whereas for polyoxyethylene tridecyl ether only DWM-1 type materials [for Cl3(EO)12] or DWM-2 [for C13(EO)6] are obtained. The different behavior is explained considering the VH/rVLratio. Of course our interpretations will not last universally as there are so many syntheses variables that have to be taken into account in such preparations. It was also found that the texture strongly depends on the hydrothermal treatment conditions. The expansion of pore size with heating time and temperature can be explained by the change of surfactant conformation with temperature and time. ACKNOWLEDGEMENT
:
This work has been performed within the framework of PAI/IUAP 4-10. Alexandre L6onard and Gontran Herrier thank FNRS (Fond National de la Recherche Scientifique, Belgium) for a FRIA scholarship.
125 REFERENCES
1.
2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13 14. 15. 16. 17. 18. 19. 20. 21.
J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.TW. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins and J.L. Schenker, J. Am. Chem. Soc., 114 (1992) 10834 C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli and J.S. Beck, Nature, 359 (1992) 710 P.T. Tanev and T.J. Pinnavaia, Chem. Mater., 8 (1996) 2068. TUD-1, Shen, Ziping; Jansen, and al., Mesoporous amorphous silicate materials and process for the seperation therof, Patent application, EU4741, (1998). Q. Huo, D.I. Margolese and G.D. Stucky, Chem. Mater., 8 (1996) 8 1147. S.A. Bagshaw, E. Prouzet and T.J. Pinnavaia, Science, 269 (1995) 1242. J.L. Blin, A. L6onard and B.L. Su, Chem. Mater., 13 (10) (2001) 3542. G.S. Attard, J.C. Glyde and C.G. GSltner, Nature, 378 (1995) 366. N.R.B. Coleman and G.S. Attard, Microporous and Mesoporous Mater., 44-45 (2001) 73. W. Zhang, B. Glomski, T.R. Pauly. and T.J. Pinnavaia, Chem. Comm., (1999) 1803. J.L. Blin, L. Gigot, A. L6onard and B.L. Su, Nanoporous III, accepted for publication. J.L. Blin, O. Provoost, A. L6onard and B.L. Su, to be published. E.P. Barret, L.G. Joyner, and P.P. Halenda, J. Am. Chem. Soc., 73 (1951) 37. D.J. Mitchell, G.J.T. Tiddy, L. Waring, T. Bostock and M.P. Mc Donald, J. Chem. Soc. Faraday Trans. 1 79 (1983) 975. L. Sierra and J.L. Guth, Microporous and Mesoporous Mater. 27 (1999) 243. H. Kunieda, K. Ozawa and K.L. Huang, J. Phys. Chem. B, 102 (1998) 83 I. G. Herrier and B.L. Su, Stud. Surf. Sci. Catal., 135 (2001) 08-0-02 G.D. Stucky, Q. Huo, A. Firouzi, B.F. Chmelka, S. Schacht, I.G. Voigt-Martin anf F. Schtith, Stud. Sure Sci. Catal., 105 (1997) 69. J.M. Kim, S.E. Park and G.D. Stucky, Stud. Surf. Sci. Catal., 135 (2001) 08-P-12 M. Kruk and M. Jaroniec, Langmuir, 15 (1999) 5279. R. Ryoo, C. H. Ko and I.S. Park, Chem. Commun., (1999) 1413.
This Page Intentionally Left Blank
Studies in Surface Science and Catalysm 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
127
M e s o p o r o u s silicas via organic-inorganic hybrids based on charged p o l y m e r s Graham M Gray and John N Hay Department of Chemistry, School of Physics & Chemistry, University of Surrey, Guildford, Surrey, GU2 7XH, England. A range of polyviologens synthesised by the Menshutkin reaction have been successfully incorporated into silica hybrids using the hydrolytic sol-gel route. Hybrids were calcined at 650~ to remove the polymer, forming porous amorphous silica products. Nitrogen adsorptiondesorption studies have been undertaken on the hybrids and the calcination products. The hybrid porosities depend on the polymer content and type and the nature of the counter-ion. Calcination leads to silicas whose porosity depends on the nature and concentration of the polyviologen (PV) used. A significant effect of the counter-ion has been noted in these systems. 1. INTRODUCTION Synthesis of silica with controlled porosity has attracted much attention recently because of the range of potential applications for the products, including their use in catalysis and as catalyst supports, in separation processes and in sensors. One route to producing this porosity is the use of small molecules or polymers incorporated into the forming silica network as structure control agents, which are subsequently removed to leave the desired porosity [ 1-3]. A variety of templates has been studied for the control of porosity in amorphous silica synthesised by the hydrolytic sol-gel route including small molecules and polymers [4], supramolecular arrays [5] and bacteria [6], which can template the growth of inorganic species via electrostatic, van der Waals and hydrogen bonding interactions, or combinations thereof. In mesoporous silica synthesis using charged surfactant templates, electrostatic interactions are believed to play a key rrle in the initial organisation of the organic-surfactant array [5]. Both polymers and oligomers have been used to synthesise a wide range of organic-inorganic hybrids by the hydrolytic sol-gel route and the polymeric species or their supramolecular assemblies can act as templates for the resulting silica structure [7,8]. Surprisingly little attention has been paid to cationic polymers [8], despite the fact that cations and cationic surfactant assemblies are used to form porous crystalline zeolites and amorphous mesoporous silicas. There is also clear evidence of the importance of functionality in controlling the structure of natural organic-inorganic hybrid materials [6,9]. Synthetic charged polymers might therefore exert a structure directing effect on the growth of sol-gel silica networks. We have previously reported our investigations into the possibility of polyviologens (bipyridinium polymers) acting as non-bonding templates during the hydrolytic sol-gel process [ 10-13]. Polyviologens are an interesting class of cationic polymer and have found use in a wide variety of fields including herbicides, electrochromism and molecular electronics. Our interest in cationic polymers as potential templates stems from the use of cations and cationic surfactants for this purpose in the formation of zeolites and amorphous silicas. As part of our continuing investigation into these materials we report here preliminary results into the possibility of the associated counter-ion playing a r61e in this process.
128 2. EXPERIMENTAL 2.1 Chemicals p-Toluenesulfonyl chloride (98%) was purchased from Aldrich and used as received. Pyridine (AR), 4,4'-bipyridine (98%), 1,3-propanediol (98%), 1,5-pentanediol (97%), 1,3dibromopropane (98%), 1,5-dibromopentane (97%) and tetramethylorthosilicate (TMOS, 98%) were purchased from Lancaster and used as received. Methanol (AR), glacial acetic acid, ethyl acetate (AR), and hydrochloric acid (sp. gr. 1.18) were purchased from Fisher and used as received. Acetonitrile (HPLC, Fisher) was freshly distilled from Call2 under an atmosphere of nitrogen before use. 2.2 Instrumentation Infra-red (IR) spectra of the polyviologens and the sol-gel hybrids (as KBr discs) were recorded on a Perkin-Elmer 1750 Fourier transform IR (FT-IR) spectrometer. IH nuclear magnetic resonance (NMR) spectra were obtained using a Bruker AC-300 NMR spectrometer operating at 300.15 MHz, using CD3OD, D20 or DMSO-d6 as a solvent. Analyses for carbon, hydrogen and nitrogen were carried out on an Exeter Analytical EA440 machine. N2 adsorption-desorption isotherms at 77 K were obtained using a Micromeritics Gemini 2375 instrument. Samples were outgassed for at least 5 hours at 120~ under N2(g). Analysis of the surface area and porosity of the hybrids and the silica products resulting from calcination was based on the method derived by Brunauer, Emmett and Teller (BET) [ 14,15]. 2.3 Synthesis of ditosylate ester monomers A slightly modified version of the procedure reported by Marvel and Sekera [ 16] was used. The preparation of 1,3-propaneditosylate is given here as an example. Pyridine (20ml) and 1,3propanediol (1.704g, 1.62ml, 22.4mmoi) were added to a 100ml RB flask equipped with a magnetic stirrer. The flask was cooled to 0~ and p-toluenesulfonyl chloride (8.701g, 45.6mmol) added in portions over 5 minutes taking care to ensure that the temperature did not rise above 15~ The mixture was stirred for 3.5 hours below 20~ before addition of hydrochloric acid (15ml) in ice-cold water (50ml). The ester that crystallised was collected on a chilled Buchner funnel and sucked as dry as possible. Recrystallisation from methanol yielded a crystalline white powder, which was then dried under vacuum at 60~ for 24 hours. Yield = 4.86g; 56%, melting point 88-89~ The purity of the monomers was checked by IH NMR (tosylates in CD3OD, bromides in D20) and elemental analysis. 2.4 Polyviologen (PV) synthesis Equimolar amounts of 4,4'-bipyridyl and the corresponding monomer (ditosylate ester or dibromoalkane) were stirred in dry acetonitrile at 80~ for 120 h under an atmosphere of nitrogen according to the previously reported procedure [3]. The resulting polymers (e.g. I) were dried under vacuum at 80~ for 24 h. Analytical data for the polyviologens are presented in tables 1-4. PPrV is polypropylviologen and PPeV is polypentylviologen. I -I-
+
~___/ TsO-
129
2.5 Synthesis of silica-polyviologen hybrids Two methods were used to synthesise the hybrids. Method 1. The order of addition of reagents was as follows. 1. PV. 2. H20. 3. MeOH. 4. Acetic acid. 5. TMOS. Upon addition of methanol, the mixture was stirred to dissolve as much polymer as possible. Upon addition of TMOS the mixture became turbid and was stirred vigorously until homogenisation occurred. The mixture was covered with perforated parafilm and left for 48 hours at room temperature during which time it gelled. The sample was then dried at 80~ for 72 h before drying at 120~ for 48 h. Method 2. This method is similar to method 1 except the order of addition of reagents was as follows. 1. PV. 2. MeOH. 3. TMOS. 4. Acetic acid. 5. H20. The mixture was covered with perforated parafilm and left for 72 hours at room temperature before drying at 80~ for 10 days. Table 1. IR data for the polyviologens containing bromide counter-ions Assignment
PPrV-Br
stretch C=N stretch -CH2 deformation C-N + stretch
PPeV-Br
1640cm -1 1410 1360cm-1 1183cm -~
and
1638cm -1 1443 and 1349cml 1175cm -I
Table 2. IR data for the polyviologens containing tosylate counter-ions Assignment ......C = N
PPrV-OTs
S t r e t c i ~ ..............i 6 3 9 c m
C-C skeletal -S=O stretch C-N + stretch
PPeV-OTs
1 ~.........................................................i 6 3 8 c m
1 ~ ...................................................
1496 and 1598cm-
1494 and 1598cm-
1
1
1121 and 1350cm-
1123 and 1352cm-
1
1
1196cm -l
1196cm l
Table 3. ~H NMR data for the polyviologens containing tosylate counter-ions Chemical shift, 8 ...PPrv-OTS . 2.28 4.77 7.2-7.6 8.4-9.2 ......................................................
i~PeV'0Ts 2.26 4.65 7.1-7.8 8.6-9.4
............................................
Assignment 3H, CH3 +N-CHE dd, 2x4H, ArH m, 8H, hetero ArH
130
Table 4. ~H NMR data for the polyviologens containing bromide counter-ions Chemical shift, 6 PPrV-Br 4.7 7.9-9.2
PPeV-Br 4.65 7.8-9.2
Assignment +N-CH2 m, 8H, hetero ArH
3. RESULTS AND DISCUSSION
3.1. PV synthesis Pale off-white/yellow solids were obtained for poly(propylviologen ditosylate) (PPrV-OTs) and poly(propylviologen dibromide) (PPrV-Br). A bright yellow solid was obtained for poly(pentylviologen dibromide) (PPeV-Br). In the case of the poly(pentylviologen ditosylate) (PPeV-OTs) however, a tacky, viscous pale-yellow gel was obtained. Efforts to yield a solid by precipitation of the polymer out a solution of methanol with the careful addition of a miscible non-solvent such as chloroform, dichloromethane or diethyl ether were unsuccessful. The viologens show interesting lyotropic liquid crystalline behaviour [ 17-20], and it is possible that the gelation arises from physical interaction caused by the lyotropism. Infrared and IH NMR analysis (tables 2 and 3, above) were consistent with the formation of a viologen polymer. The addition of sodium dithionite to a solution of the polymer in methanol, which resulted in the characteristic deep blue-violet colour of the radical cation species (below, eqn 1.), also provided confirmation of the viologen structure.
--+N~-~N
m Equation 1
IH NMR spectroscopy showed that a small amount of methanol was contained within the gel despite attempts to remove it by drying under vacuum at elevated temperature. The small amount of methanol present was not deemed to be a problem, as the polymer would subsequently be dissolved in methanol during the sol-gel process.
3.2. Sol-gel hybrids The synthesis conditions for the sol-gel hybrids are reported in table 5. In each case a transparent or slightly translucent hybrid was produced suggesting a mainly nanoscale morphology.
3.3. Surface area analysis of the hybrids and calcined materials A number of factors (such as monomer concentration, r value and temperature) can influence the surface area, pore volume, porosity and pore sizes of silica xerogels. However, we have previously shown that despite the differences in r value used in the synthesis of these hybrids, it is possible to draw rational conclusions from observations of the effect of incorporation of the polyviologen in varying amounts into the sol-gel matrix [12]. The results of the present study, shown in tables 5 and 6, are broadly in agreement with our earlier predictions and observations
131 [ 12]. The previous work showed that mesoporous hybrids were formed, but with low porosities at high PV content. The present work confirms that incorporation of polyviologen within the silica matrix leads to a reduction in surface area, pore volume and porosity. All hybrids have an average pore diameter in the range 19-20)k, except for PPeV-OTs (50%), which has an average pore diameter of 22.5A. A full pore size distribution is still to be determined. Calcination of the hybrid materials at 650~ for 24 hours to remove the polyviologen leads to a decrease in surface area and total pore volume due to ageing of the, silica except when a high concentration of polyviologen was used (as seen in the previous study). In such cases, the removal of the PV has a greater effect than the ageing of the silica network resulting in an increase in the surface area and pore volume. In all cases, the average pore diameter decreases following calcination, with the most significant reduction in the case of the PPeV-OTs (50%) hybrid. Ongoing work will confirm whether or not the calcined silicas show high mesoporosities, as seen previously. Of interest is the difference in surface area and pore volume for the incorporation of polyviologens at similar loading but with different counter-ions. It is known that the choice of counter-ion can infuence the polymer properties [21-23]. Harris and co-workers have shown that replacing the tetrafluoroborate counter-ion in poly(pyridinium tetrafluoroborate)s with the triflate anion (known for its thermal stability) leads to a significant increase in thermal and thermo-oxidative stability [21,22]. Bhowmik and co-workers noted that by reducing the strong interaction between positive and negative charges compared to an inorganic counter-ion, the presence of a bulky organic counter-ion increased solubility in methanol and dimethylsulphoxide to the extent that formation of a lyotropic liquid crystalline phase was possible [23]. The presence of the different counter-ions used in this study (Br and TsO) is also likely to lead to differences in polymer packing due to the steric effect of a large bulky tosylate anion compared to the bromide ion. As the growing silica network forms around the polymer chains during the sol-gel process it is possible that such differences in packing of the polymer would be maintained in the resultant sol-gel hybrids. This could account for the marked differences in the surface area and pore volume of the sol-gel hybrids containing the same loading of polymer but with a different counter-ion. A more systematic study is required to confirm these results and, if possible, quantify the effect of different counter-ions. Table 5. Synthesis and surface area data for the sol-gel hybrids PV used (weight%)
Method
r
rs
ra
Gelation time
PPrV-Br (10%)
1
7.8
0.1
0.5
<16h
pale yellow, transparent
129
0.070
PPrV-OTs (10%)
2
4.1
7.3
0.99
22h
colourless, transparent
348
0.188
PPeV-Br (10%)
1
5.8
0.1
0.5
<16h
colourless, transparent
87
0.047
PPeV-OTs (10%)
2
3
2
0.99
<24h
yellow, translucent
394
0.214
2
0.99
<24h
yellow, translucent
64
0.040
PPeV-OTs 2 8.2 (50%) r - water:alkoxide ratio rs = solvent:alkoxide ratio ra = acid:alkoxide ratio
Appearance
BET surface area
Total pore volume
132 Table 6. Surface area data for the calcined materials PV used
BET surface area
Total pore volume (Vp)
PPeV-OTs (10%) PPeV-OTs (50%) PPrV-Br (10%)
250 385 56
0.132 0.210 0.030
4. A C K N O W L E D G E M E N T S The UK Engineering and Physical Sciences Research Council (EPSRC) is thanked for funding. Elemental analyses were carried out by Ms. N. Walker.
5. REFERENCES
1. Helmkamp, M. M.; Davis, M. E. Ann. Rev. Mater. Sci. 25 (1995) 161. 2. Burkett, S. L.; Davis, M. E. Chem. Mater. 7 (1995) 1453. 3. Davis, M. E.; Chen, C.-T.; Burkett, S. L.; Lobo, R. F. Mat. Res. Soc. Symp. Proc., 346 (1994) 831. 4. Raman, N. K.; Anderson, M. T.; Brinker. C. J. Chem. Mater. 8 (1996) 1682. 5. Dabadie, T.; Ayral, A.; Guizard, C.; Cot, L.; Robert, J. C.; Poncelet, O. Mat. Res. Soc. Symp. Proc., 346 (1994) 849. 6. Davis, S. A.; Burkett, S. L.; Mendelson, N. H.; Mann, S. Nature 385 (1997) 420. 7. Sommerdijk, N. A. J. M.; van Eck, E. R. H.; Wright, J. D. Chem. Commun. (1997) 159. 8. Sato, S.; Murakata, T.; Suzuki, T.; Ohgawara, T. J. Mater. Sci. 25 (1990) 4880. 9. Heuer, A. H.; Fink, D. J.; Laraia, V. J.; Arias, J. L.; Calvert, P. D.; Kendall, K.; Messing, G. L.; Blackwell, J.; Rieke, P. C.; Thompson, D. H.; Wheeler, A. P.; Veis, A., Caplan, A. I. Science 255 (1992) 1098. 10. Adeogun, M. J.; Hay, J. N. Polym. Int. 41 (1996) 123. 11. Adeogun, M. J.; Fairclough, J. P. A.; Hay, J. N.; Ryan, A. J. J. Sol-Gel. Sci. Tech. 13 (1998) 27. 12. Adeogun, M. J.; Hay, J. N. Chem. Mater, 12 (2000) 767. 13. Adeogun, M. J.; Hay, J. N. J. Sol-Gel Sci. Techol. 20 (2001) 119. 14. Gregg, S. J.; Sing, K. S. W. Adsorption, Surface Area and Porosity;, Academic Press: London, 1967. 15. Lowell, S.; Shields, J. E. Powder Surface Area and Porosity, 3rd Ed.; Chapman and Hall: London, 1991. 16. Marvel, C. S.; Sekera, V. C. in Organic Syntheses Collect. Vol. III, Wiley: New York, 1955, pp.366-367. 17. Han, H. S.; Bhowmik, P. K. TRIP 3 (1995) 199. 18. Bhowmik, P. K.; Han, H. S. J. Polym. Sci., Polym. Chem. Ed. 33 (1995) 1745. 19. Bhowmik, P. K.; Akhter, S.; Han, H. J. Polym. Sci., Polym. Chem. Ed. 33 (1995) 1927. 20. Bhowmik, P. K.; Xu, W.; Han, H. S. J. Polym. Sci., Polym. Chem. Ed. 32 (1994) 3205. 21. Harris, F. W.; Chuang, K. C.; Huang, S. A. X.; Janimak, J. J.; Cheng, S. Z. D. Polymer 35 (1994) 4940. 22. Huang, S. A. X.; Chuang, K. C.; Cheng, S. D.; Harris, F. W. Polymer 41 (2000) 5001. 23. Bhowmik, P. K.; Burchett, R. A.; Han, H.; Cebe, J. J. J. Polym. Sci. Part A Polym. Chem. 39 (2001) 2710.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
133
M e s o p o r o u s silicas o f hierarchical structure b y h y d r o t h e r m a l s u r f a c t a n t - t e m p l a t i n g under m i l d alkali conditions Zhong-Yong Yuan, a,b Wuzong Zhou, c Bao-Lian Su a,. and Lian-Mao Peng b Laboratory of Inorganic Materials Chemistry, ISIS, The University ofNamur (FUNDP), 61 rue de Bruxelles, B-5000 Namur, Belgium. e-mail:
[email protected] a
b Beijing Laboratory of Electron Microscopy, Institute of Physics & Center for Condensed Matter Physics, Chinese Academy of Sciences, P.O. Box 2724, Beijing 100080, China c School of Chemistry, University of St. Andrews, St. Andrews, Fife KY16 9ST, UK
Mesoporous silicas with hierarchical structures were synthesized under a mild alkali condition by cationic or mixed cationic-nonionic surfactant templating. When cetylpyridium bromide was used, a novel morphology of mesoporous silica of type MCM-41 was formed. It was obsearved that single nanotubes with diameter of about 5 nm and bundles of nanotubes grew from the (001) surface of the mesoporous silica particles, forming a paintbrush-like morphology. The synthesis process was investigated and the formation mechanism of such a surface nanotube patterning is discussed. When mixed surfactant of cetylpyridium chloride and Triton X-100 was used, a mixed ordered-disordered hierarchical mesostructure with arc rings of submicrometer scales was observed in the synthesized mesoporous silica which exhibits a narrow pore size distribution, high surface area and a large pore volume. Arc ropes consisting of ordered mesopores, as well as many spheres of submicrometer in diameter with shells of about 40 nm in thickness consisting of ordered arrays of mesopores, were observed, though the majority of the particles contained disordered mesoporous microdomains. This material lacks overall long-range ordering whereas local ordering of mesopores exists.
1. INTRODUCTION A variety of ordered mesoporous materials have been synthesized using supramolecular assembly of surfactant molecules as a template since the appearance of mesoporous M41S [1,2]. These materials have a range of framework compositions, morphologies, and porous structures. Correspondingly a number of models have been proposed in order to explain the formation of mesoporous materials and to provide a rational basis for the various synthesis routes [3,4]. Many efforts have been devoted recently to the macroscopic morphological control of mesoporous silicas, since it is now apparent that morphological control and texture of mesoporous silicas are extremely important for diverse industrial applications [5,6]. Syntheses of mesoporous silicas in various forms, such as films, fibers, spheres, monoliths, curved shapes, and designed patterns, have been achieved using the surfactant-templating method often under relatively wild conditions (such as strongly acid and basic media) [6-12]. On the other hand, mixed surfactants have been used as mixed micellar templates for the synthesis of mesoporous silicas with tailored properties [13-15]. The pore size of mesoporous silicas could be fine controlled by using the mixed surfactant with various ratios [13,16].
134
Mesoporous silica spheres have been synthesized with mixed cationic-nonionic surfactant under a strong acidic condition [ 14]. Cubic silica MCM-48 has been obtained in the presence of either mixed cationic-neutral surfactant [15] or mixed cationic-anionic surfactant micelles [17], respectively, under alkaline conditions. We have synthesized silica-based mesoporous materials with hierarchical structures under a mild alkaline condition by cationic or mixed cationic-nonionic surfactant templating. Surfactant cetylpyridium and Triton X-100 were used. NH4OH was used to tune the alkaline of the synthetic gel. A novel surface nanotube pattern grew on MCM-41 particle surface by single cationic surfactant templating. Whileas a mixed ordered-disordered mesostructure with arc rings of submicrometer scales was observed in mesoporous silica materials synthesized with mixed surfactants.
2. E X P E R I M E N T A L Cetylpyridinium bromide (CPBr) was used as a single cationic surfactant template. In a typical synthesis experiment, 5.76 g of CPBr was dissolved in 70 ml of water, 18.8 ml of NHnOH (25%) was then added under stirring, resulting in a clear solution. Then, 6.26 g of tetraethoxysilane (TEOS) was added slowly with stirring. The pH value of the final mixture was about 9.2. After further stirring for 30 min, the mixture was loaded into an autoclave and statically heated at 80 ~ for 72 h. The resultant solid product was recovered by filtration, washed with distilled water and dried in air at ambient temperature. The as-synthesized material was heated in air with temperature increased from room temperature to 540 ~ at a rate of 1 ~ and was then calcined at 540 ~ for 5 h. Cetylpyridinium chloride (CPC1) and Triton X-100 were used in the mixed surfactant templating. The typical synthetic conditions are as follows. 1.07 g of CPC1 and 2.43 g of Triton X-100 were dissolved in 15 ml of NH4OH (25%) and 50 ml of water. To this solution, 3.13 g of TEOS was added at room temperature with stirring. After further stirring about 45 min, the mixture was allowed to crystalline at 90 ~ for 72 h in a stainless-steel autoclave. Powder X-ray diffractograms (XRD) of the solids were recorded on a Rigaku D/max 2400 diffractometer using CuK~ radiation and scanning between 1.5~ and 10~ (20). N2 adsorptiondesorption isotherms were obtained at liquid nitrogen temperature on a Quantachrome Autosorb1 apparatus. The sample was outgassed at 300 ~ over 10 h prior to adsorption. The specific surface area was determined by the BET (Brunauer-Emmett-Teller) method and the pore-size distribution was obtained from the N2 adsorption isotherm using the BJH (Barrett-JoynerHalenda) method. Transmission electron microscopy (TEM) was carried out on a Jeol JEM2010 electron microscope operating at 200 kV. The specimens for the TEM studies were prepared by dispersing the particles in alcohol by ultrasonic treatment, and dropping onto a holey carbon film supported on a copper grid.
3. RESULTS AND DISCUSSION
3.1. Single cationic surfactant templating The X-ray diffraction patterns of mesoporous silicas synthesized with single surfactant exhibit at least four diffraction peaks in the 20 range of 2 to 7~ (Figure 1), reflecting a typical MCM-41 mesostructure [1,2]. After calcination, only a very small decrease of the hexagonal unit cell parameter from 5.10 to 5.00 nm was detected, suggestive of the high thermal stability of mesoporous silicas synthesized under the present condition [ 18]. All samples exhibit a surface area of more than 1000 m2/g, as calculated from low-temperature N2 adsorption-desorption
135
isotherms with typical irreversible type IV [19]. The nitrogen adsorption usually shows a typical rectangular hysteresis loop, as previously reported elsewhere [18]. This hysteresis shape represents a uniform tubular capillary pore calcined geometry with wide and narrow regions in the pore channels. The corresponding uniform pore size is about 3.1 nm. ~ as-synthesized A novel morphology of the surface when viewed down a direction I perpendicular to the pore axis has 10 2 4 6 8 been revealed. Many single silica 20 (degree) nanotubes and bundles of single Figure 1. Typical XRD pattems of mesoporous nanotubes appear on the (001) silicas by single cationic surfactant templating. surfaces of the particles (Figure 2). The diameter of a single nanotube is about 5 nm. The average diameter of the bundles of nanotubes is about 20 - 4 0 nm. All the silica nanotubes are parallel to the mesopore axis of the MCM-41 structure, though some nanotubes are bent. The lengths of the nanotubes were almost uniform in the same sample, and could be varied with the synthesis time (Figure 2). The surface nanotube patteming existed after 60-hour hydrothermal treatment, and the nanotubes could continue growing with the increase of crystallization time. The formation of the nanotubes was markedly enhanced after keeping for 72 h at 80 ~ The length of the nanotubes could reach above 250 nm after 80 h of hydrothermal treatment. Single nanotubes were also observed in Figures 2 and 3. Such a paintbrush-like morphology was maintained after calcination at 540 ~ for removing the organic templates [18]. According to a previous TEM study of MCM-41 specimens at different stages of formation, it was found that diffusion process of chemical spieces in the solution and in the surfactant-silica particles is important [20,21 ]. The initial nuclei of mesoporous silica were formed even before the hydrothermal treatment. However the surface of the mesostructured silicate-surfactant composite particle was rough and less condensed. The collected mixed gel, after roomtemperature stirring without any hydrothermal treatment, gave a well-defined X-ray diffraction pattern, characteristic of MCM-41, with a small dl00 spacing less than 3.48 nm. The hexagonally ordered mesopores were observed directly by TEM. During the hydrothermal treatment, the initial mesostructured silicate-surfactant composite particles could be restructured, forming better ordered array of mesochannels with larger dl00 spacing (4.09 nm), which can be confirmed by the XRD and TEM data. There are still silicate species and surfactant micelles in the precursor solution as detected by ~H, 13C and 29Si MAS NMR. Those partially hydrolyzed TEOS would continue to aggregate with the surfactant micelles to generate condensed rods during the mild hydrothermal treatment, and the condensation stabilizes the rods. While the spherical end cap of the cylindrical rod is relatively unstable due to the lack of geometric matching [22], which would proceed on the surface of initial mesostructured silica nucleus particles and connect together by the geometric matching between the occupied area of surfactant molecules and silicate molecules respectively, and thus the mesochannels would elongate from the initial silica particle surface during crystallization. On the other hand, due to the flexibility of surfactant micelle rods, the growth of mesochannels might be anisotropic. The growth direction of every nanotube could be different, even bent. And several nanotubes could linked together during growth, forming some small bundles of nanotubes on the surface. Thus, it
}
I
,
I
I
I
i
I
i
136
Figure 2. Typical TEM images of the as-synthesized mesoporous silicas of MCM-41 type, showing paintbrush-like (001) surface patterning: (a) short nanotube patterning by 72 hours of crystallization and (b) longer nanotubes after 80 hours of crystallization
Figure 3. TEM image of the as-synthesized mesoporous silicas showing several short nanotubes growing from the particle surface
137 is possible to form the present surface patterning of nanotubes. This proposed formation mechanism of surface nanotube patteming could be supported by the TEM images at the initial stage of nanotube growing (Figure 3). Figure 3 shows several short nanotubes growing from the particle surface, and its direction is parallel to the mesopore axis of the mesostructure. The particle surface is rough due to the growing of nanotubes. Such morphology was not found in the initial mesostructured silica particles before hydrothermal treatment. That is to say, hydrothermal treatment is necessary for the formation of this novel surface patteming. Another possible support is from very recent report of Mokaya [23] who investigated the effect of increasing the time of hydrothermal crystallisation during high temperature (150 ~ synthesis of MCM-41. A change of morphology from spherical particles to elongated or rope-like particles was found, and micrometre sized MCM-41 'ropes' made up of smaller silica fibres were obtained after long time of crystallization (168 h). A recent report of Lin et al. [24] also presented the mesoporous silica nanotubes obtained by post-synthesis hydrothermal treatment of their acid-made mesoporous silicas. The diameter of tubes was around 30-100 nm. The formation mechanism of the transformation of surfactantsilica interactions was proposed. Obviously, the mechanism of our nanotubes' formation should be quiet different with theirs. The present work can supply interesting information on the understanding of the mesostructure formation mechanism. Moreover, transition metal ions Ti and V have been introduced into the MCM-41 mesoporous materials, and the paintbrush-like morphology remained unchanged [ 18,25].
3.2. Mixed surfactant templating The molar composition of the synthetic gel with mixed surfactant templating is 1 TEOS : 14.6 NH4OH : 0.2 CPC1 : 0.25 TX-100 : 185 H20. The powder X-ray diffraction pattern of the as-synthesized material shows some overlapped reflections in the low 20 angle range with very low intensity (Figure 4a). However, after calcination, an intense peak corresponding to a dspacing of 4.1 nm presented together with another broad peak around 2.2 nm of d-spacing (Figure 4a). This pattern is characteristic of a mesophase, but it is different from those of either the ordered MCM-41 [ 1] or the disordered materials, for instance KIT- 1 [26] made with cationic surfactant in the presence of organic salts and MSU-n [27] prepared by nonionic surfactant templating. The latter materials generally display single dl00 reflections indicative of uniform worm-like mesopores without long-range periodicity [27]. Compared to the XRD patterns of MCM-41 with hexagonally ordered channels, the present calcined sample might have a novel pore structure, but with lower degree of structural ordering. The arising of the reflection peaks of 4.1 and 2.2 nm of d-spacing on the XRD pattern for the calcined sample suggests that during the calcination a relatively ordered array of well-defined mesopores was formed. It is believed that, in the as-synthesized material, mesopores filled with templating molecules already existed but in a disordered manner. The mesopores may be rearranged into a more ordered form during calcination to remove the templating molecules from the pores. The nitrogen adsorption-desorption isotherm of the calcined product and its corresponding BJH pore-size distribution curve are presented in Figure 4b. A typical irreversible type IV adsorption isotherm with a hysteresis loop, as identified by IUPAC [19], is seen. A well-defined step occurs in the adsorption curve at a relative pressure P/Po of ca. 0.35, which is indicative of the filling of framework-confined mesopores. The P/P0 position of the inflection points is clearly related to a diameter in the mesopore range and the step indicates the mesopore-size distribution. The pore-size distribution curve shows a narrow peak centered at 3.2 nm. The BET surface area is 1142 mR/g, and the single-point total pore volume at a relative pressure of 0.978 is 1.232 cm3/g. TEM images of the mixed-surfactant-templated silica samples are shown in Figure 5. It was found that the majority of the particles contain disordered mesoporous microdomains. Two arc
138 ropes, consisting of ordered mesopores, are present in one monolith (Figure 5a). We can also see in Figure 5b many spheres of about 390 to 700 nm in diameter, with shells of approximately 40 nm in thickness, which consist of ordered arrays of mesopores similar to those in Figure 5a. However, ordered array of mesopores was only observed in these arc rings. Such a disorderedordered mesostructure has not been reported in the literatures to date, to the best of our knowledge. Although some of vesicle structures have been reported to present occasionally under a similar mild alkaline condition [25], the shell of the vesicles previous reported was composed of disordered mesotubules.
(a) 80(} (b_,)_Adsorption 700~. -" Desorption j
f
"~ 60~
40 -~ I[ I ~
as.'s~~ynthesized .... 20
1oo
]
2
4
6 8 20 (degrees)
10
0.0
"2
Pore size (nm)
0.2 0.4 0.6 0.8 1.0 Relative pressure (P/Po)
Figure 4. (a) Powder XRD patterns of synthesized samples using mixed surfactant templates; (b) N2 adsorption-desorption isotherm and the pore size distribution (inset) of the calcined samples. If single cationic surfactant CPCI was used in the synthesis, one well-defined hexagonal mesoporous MCM-41 could be obtained [13,28]. On the other hand, lamellar mesophase may be produced when neutral surfactant alkylamine was used in this mild alkaline system. However, no significant yield of mesostructural products could be synthesised when nonionic surfactant Triton X-100 was used as the only template in the given synthetic system. If nonionic surfactant was initially protonated under low pH conditions, followed by base catalyzed neutralization in order to increase pH value in the solution to certain threshold values (between 5 and 6), mesoporous silicate MSU-2 possessing non-symmetrical worm-like pores could be synthesized. This synthetic route was labeled as N~ - (where N O stands for nonionic surfactant, M + for Na + or NH4+, and I- for hydroxylated tetraethyl orthosilicate) [29]. Sodium silicate solutions can also be used to synthesize mesoporous silicas by their addition to an acidic Triton X-100 solution (pH around 2), followed by a pH adjustment using NaOH or NHaOH to the value required for the polycondensation (usually between 6 and 7) [30]. It has been revealed that mesoporous silicas templated by cationic surfactants (S+) under basic conditions are produced by a S+I pathway where anionic silicate precursors (I) are assembled at the interface of rod-like micelles through electrostatic interactions, resulting in a hexagonal mesostructure [31]. Whereas mesoporous silicas templated by nonionic poly(ethylene oxide) (PEO)-based surfactants (N~ under neutral conditions are synthesized by a neutral N~ Otemplating pathway where neutral silica precursors (I~ are assembled at the interface of flexible worm-like micelles by hydrogen bonding, resulting in a disordered mesostructure [26].
139 However, in the present basic solution, the neutral surfactant N o should combine with the cationic surfactant S+ and with the anionic inorganic species to form a complex surfactant-silica mesophase, since these completely miscible surfactants exhibit complex phase behaviors in aqueous solutions [32] forming liquid-crystalline micellar mesophases cooperatively. Thus, the mesoporous silica synthesized by mixed cationic-nonionic surfactant templating under the present basic condition might form via a complex templating pathway: (S+N~ (M+ NH4+) and could be referred to a modified formation mechanism. The resultant ordered-disordered mesostructure could be affected by the ratio of the nonionic to cationic surfactants, and could be regarded as an intermediate structure between the ordered hexagonal MCM-41 and a disordered mesostructure. Since the nonionic/cationic surfactant ratio is larger than 1 in the present study, we believe that nonionic surfactant Triton X-100 must play an important role in the synthesis of the present complex mesostructure. In summary, mesoprous silicas with disordered-ordered hierarchical mesostructure has been synthesized by mixed cationic-nonionic surfactant templating under mild alkaline conditions. The present results demonstrate that mixed cationic-nonionic surfactant templating route can provide a suitable approach for the synthesis of silica-based mesoporous molecular sieves. It is certainly true that the synthesis has not yet been optimized. Further improvement of the synthetic method and studies of the relationship between the structure and the properties of these new mesoporous materials are currently carried out in these laboratories. =
Figure 5. TEM micrographs of calcined silicas showing disordered-ordered mesostructure.
140 4. ACKNOWLEDGEMENT This work is financially supported by the National Natural Science Foundation of China (NSFC), Chinese Academy of Sciences, and the Belgium Federal Government PAI-IUAP 4/10 project. REFERENCES
1. C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli, and J.S. Beck, Nature, 359 (1992) 710. 2. J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T.-W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins, and J.L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. 3. A. Sayari, and P. Liu, Microporous Mater., 12 (1997) 149. 4. J.Y. Ying, C.P. Mehnert, and M.S. Wong, Angew. Chem. Int. Ed., 38 (1999) 56. 5. D. Zhao, P. Yang, Q. Huo, B.F. Chmelka, and G.D. Stucky, Curr. Opin. Solid State Mater. Sci., 3 (1998) 111. 6. H. Yang, N. Coombs, and G.A. Ozin, Nature, 386 (1997) 692. 7. H. Yang, G.A. Ozin, and C.T. Kresge, Adv. Mater., 10 (1998) 883. 8. S.M. Yang, H. Yang, N. Coombs, I. Sokolov, C.T. Kresge, and G.A.Ozin, Adv. Mater., 11 (1999) 52. 9. S.M. Yang, I. Sokolov, N. Coombs, C.T. Kresge, and G.A. Ozin., Adv. Mater., 11 (1999) 1427. 10. Q. Huo, J. Feng, F. Schfith, and GD. Stucky, Chem. Mater., 9 (1997) 14. 11. H.-P. Lin, and C.-Y. Mou, Science, 273 (1996) 765. 12. P. Yang, D. Zhao, B.E Chmelka, and GD. Stucky, Chem. Mater., 10 (1998) 2033. 13. D. Khushalani, A. Kuperman, N. Coombs, and G.A. Ozin, Chem. Mater., 8 (1996) 2188. 14. L. Qi, J. Ma, H. Cheng, and Z. Zhao, Chem. Mater., 10 (1998) 1623. 15. R. Ryoo, S.H. Joo, and J.M. Kim, J. Phys. Chem. B, 103 (1999) 7435. 16. R. Ryoo, C.H. Ko, and I.-S. Park, Chem. Commun., (1999) 1413. 17. F. Chen, X. Yan, and Q. Li, Stud. Surf. Sci. Catal., 117 (1998) 273. 18. Z. Yuan, and W. Zhou, Chem. Phys. Lett., 333 (2001) 427. 19. K.S.W. Sing, D.H. Everett, R.A.W. Haul, L. Moscow, R.A. Pierotti, J. Rouquerol, T. Siemieniewska, Pure Appl. Chem. 57 (1985) 603. 20. W. Zhou, and J. Klinowski, Chem. Phys. Lett., 292 (1998) 207. 21. W. Zhou, R. Mokaya, Z. Shan, and T. Maschmeyer, Prog. Nat. Sci.; 11 (2001) 33. 22. M. Adachi, T. Harada, and M. Harada, Langmuir, 16 (2000) 2376. 23. R. Mokaya, Microporous Mesoporous Mater., 44-45 (2001) 119. 24. H.P. Lin, C.Y. Mou, S.B. Liu, Adv. Mater., 12 (2000) 103. 25. Z.Y. Yuan, W.Z. Zhou, Z.L. Zhang, J.Q. Liu, J.Z. Wang, H.X. Li, and L.-M. Peng, Surf. Interface Anal. 32 (2001) 193. 26. R. Ryoo, J.M. Kim, C.H. Ko, and C.H. Shin, J. Phys. Chem., 100 (1996) 17718. 27. S.A. Bagshaw, E. Pouzet, and T.J. Pinnavaia, Science, 269 (1995) 1242. 28. Z.Y. Yuan, W. Zhou, L.M. Peng, J.Z. Wang, and H.X. Li, Stud. Surf. Sci. Catal., 135 (2001) 979. 29. S.A. Bagshaw, T. Kemmitt, and N.B. Milestone, Microporous Mesoporous Mater., 22 (1998) 419. 30. L. Sierra, B. Lop6z, H. Gil, and J.-L. Guth, Adv. Mater., 11 (1999) 307. 31. Q. Huo, D.I. Margolese, U. Ciesla, P. Feng, T.E. Gier, P. Sieger, R. Leon, P.M. Petroff, F. Sch/ith, and GD. Stucky, Nature, 368 (1994) 317. 32. P.M. Holland and D.N. Rubingh, Surfactant Sci. Ser., 37 (1991) 141.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rightsreserved.
141
Synthesis and characterisation o f super-microporous aluminosilicates prepared via primary amine templating Emesto Bastardo-Gonzalez, a Robert Mokayab and William Jones a aDepartment of Chemistry, University of Cambridge, Lensfield Road, Cambridge CB2 1EW, U.K.
bSchool of Chemistry, University of Nottingham, University Park, Nottingham NG7 2RD, U.K.
Super-microporous aluminosilicate catalysts, possessing pores in the range 14 - 20A, can be prepared via primary amine templating alone or in combination with post-synthesis A1 grafting. Post-synthesis grafting of extra A1 also serves to remarkably improve the acidity and catalytic activity of the materials. Preparation of the super-microporous materials is made possible by circumventing the limitation on the lowest pore size obtainable, during supramolecular templating with primary amines, by improving the incorporation of A1. This is achieved by ensuring optimum dissolution of the A1 source and the formation of Al-rich aluminosilicate precursors prior to addition of the primary amine template. Performing postsynthesis grafting of extra A1 reduces the pore size of the resulting materials further thus increasing the possible pore size range. The super-microporous aluminosilicates are structurally as well ordered as any other primary amine templated mesoporous aluminosilicate materials. 1. INTRODUCTION The synthesis of porous inorganic materials, which may be used as heterogeneous catalysts, adsorbents or as hosts for composite materials is currently attracting a great deal of interest in materials science research. The ability to tailor the nanostructure and in particular the pore size of ordered inorganic solids is a key factor in their use in areas such as catalysis and molecular separation. For example the design and synthesis of materials that have a well defined pore structure similar to that of zeolites, but with larger pores has been a main research goal in solid acid catalysis over the past decade [ 1]. Recent advances, which include the synthesis of the M41S family of mesoporous solids [2], have to some extent achieved this goal. Many other varieties of mesoporous materials, with pores of size typically above 25A have been prepared [3]. Until recently, much less attention has been given to the synthesis of materials with pores in the super-microporous (10 - 20A) range. Solid acid materials in this pore size range are important since they bridge the gap between raditional microporous zeolites and mesoporous materials. Furthermore in addition to being able to handle molecules that are too large to be processed by zeolites, super-microporous solid acids are expected to exhibit interesting shape and size selectivity in the conversion of such molecules. Shape and
142 size selectivity is a desirable property that is generally lacking in mesoporous materials due to their larger pores. In general, supramolecular templating is used in the preparation of mesoporous materials while microporous materials are synthesised via molecular templating. Recently there have been several reports on the use of supramolecular assemblies of surfactants to template the formation of mesostructured materials with pores in the micropore and supermicropore range. Bagshaw and Hayman [4] used o~-hydroxy-bolaform surfactants to template the formation of super-microporous silicas. They obtained porous silica materials with pores in the 14 - 21 A range and pore symmetries bearing similarity to Lot, SBA-2 (P63/mmc) and M a (cram) phases. Zhao et al [5] reported the preparation of MCM-41 materials with tailored (narrow) pore openings in the super-microporous range. On the other hand Sun et al [6] used adamantanamine as templating agent for the synthesis of amorphous microporous silica and Serranno et al [7] employed cetyltrimethylammonium or dodeytrimethylammonium ions for the formation of microporous aluminosilicate materials. We have recently reported a preliminary account of the primary amine templated synthesis of super-microporous aluminosilicate materials whose pore size can be further tailored via postsynthesis grafting of A1 [8]. A further advantage of the post-synthesis grafting of extra AI is that it also serves to remarkably improve the acidity and catalytic activity of the materials. Here we report in detail the preparation, characterisation and properties of such primary amine templated super-microporous aluminosilicates. We have previously reported on the preparation of primary amine templated mesoporous aluminosilicates (AI-MMS, A1-HMS) [9-11 ]. Our previous work has shown that
the pore size of A1-MMS (A1-HMS) materials is to some extent dependent on the alkyl chain length of the primary amine template with longer amines resulting in larger pores [12,13]. The pore size was also found to be dependent on the Si/AI ratio, i.e., pore size reduced at low Si/A1 ratios [9-13]. This meant that pore sizes at the lower end of the mesopore range (-~20A) were only obtainable for highly aluminous samples and that pores in the super-microporous range (10 -20A) could not be achieved even at Si/A1 ratios as low as 7 [9-13]. Here we show that it is possible to circumvent the limitation on the lowest pore size obtainable by improving the incorporation of AI. This is achieved by modifying our previous synthesis procedure [ 11 ] so as to ensure optimum dissolution of the A1 source. Furthermore performing post-synthesis grafting of extra AI can reduce the pore size of the resulting materials further. 2. MATERIALS AND METHODS 2.1. Materials The synthesis procedure used was as follows; desired quantities of aluminium isopropoxide (AI(i-CaH70)3) were dispersed in 35 ml of isopropanol with vigorous mechanical stirring at 70~ for 15 minutes in order to dissolve the highest possible amount of the aluminium source. The resulting solution was cooled to room temperature and then added under magnetic stirring to a solution of 0.2 mol. tetraethyl orthosilicate (TEOS) in 80 ml of absolute ethanol. The resulting mixture was then heated at 70~ under vigorous stirring for 4 hours to obtain the polymerised Si-O-A1 species. After cooling to room temperature (under stirring) the inorganic precursor was added to a clear solution of 0.05 mol dodecylamine
143 (DDA) in a mixture of 80 ml of deionised water and 120 ml of absolute ethanol under slow stirring. The stirring was maintained for 5 minutes after which the resulting mixture was allowed to age at room temperature for 20 hours. The solid product was obtained by filtration, washed with two portions of 100 ml of ethanol, air-dried overnight at room temperature and finally calcined in air at 650~ for 4 hours. This procedure was used to prepare aluminosilicate materials with Si/AI molar ratios of 40:1, 20:1, 10" 1 designated AIMMSX where X is the synthesis gel Si/A1 ratio.
Grafting; Al-grafiing was performed on the A1-MMSX samples as follows; 1.28 g of a solution of chlorhydrol ([A12Cl(OH)5.2H20], 6.4 mole 1"l with respect to aluminium) was dissolved in 50 ml of distilled water and stirred at 80~ for 1 hour. 1.0 g of A1-MMSX was added to the solution and the resulting suspension stirred for another hour at 80~ After cooling to room temperature, the solid was filtered and washed with distilled water until free of CI" ions, dried in the oven at 100~ and finally calcined at 500~ for 4 hours. The resulting Al-grafted materials were designated A1A1-MMSX.
2.2. Characterisation Powder X-ray diffraction (PXRD) pattems were recorded using a Philips PW 1710 diffractometer. A graphite monochromator and CuKa radiation ()~ = 1.5418 A) were used with a Ni filter for KB attenuation. A step size of 0.02 degrees (2 theta) and a scan rate of 2 seconds per step were used. Elemental compositions were obtained using X-ray fluorescence (XRF). Surface area, pore volume and pore size were determined at -196~ by nitrogen sorption, using a micromeritics ASAP 2400 sorptometer or Coulter SA3100 sorptometer. Before analysis the samples were oven dried at 120~ and degassed at 200~ for at least 5 hours. The surface area was calculated using the BET method based on adsorption data in the partial pressure (P/Po) range 0.05 to 0.2 and the total pore volume was determined from the amount of N2 adsorbed at a P/Po = ca. 0.99. The Barrett-Joyner-Ha!enda (BJH) method and tplot analysis were used to determine the pore size and micropore surface area and pore volume.
Acidity measurement; The acid content was obtained by thermogravimetric analysis, following the adsorption of cyclohexylamine (CHA) on the samples under study. Samples were exposed to cyclohexylamine at room temperature for 16 hours and then heated in an oven at 100~ for 4 hours in order to remove any physisorbed amine. TGA curves were obtained for the CHA-containing samples using a Polymer Laboratories TG 1500 analyser with a heating rate of 20~ under nitrogen flow of 25 ml/min. The weight loss between 240 and 420~ was used to calculate the acid content assuming that each molecule of base interacts with one acid site. Catalytic evaluation; Two reactions were used to evaluate the catalytic activity of the study materials; cumene conversion and the alkylation of toluene. Conversion of cumene was performed in a tubular stainless steel, continous flow fixed-bed microreactor system with helium as carrier gas at 300oc and WHSV of 5.5. The catalyst bed (100 mg; 30-60 mesh) was first activated for 1.5 hours at, 500~ under helium (25 ml/min). During the reaction, a stream of cumene vapour in helium was generated using a saturator at room temperature. The reaction products were separated and analysed using a Carlo Erba HRGC 5300 gas chromotograph. Gas chromotographs were obtained automatically on
144 samples of the product stream which were collected at regular intervals using a Valco 6-port valve. The gas chromatographs were used to calculate the extent of cumene conversion which was principally to propene and benzene with only small amounts of t~-methylstyrene. The reaction products indicated that, under the reaction conditions used, Bronsted acid sites were the active sites. To evaluate both Bronsted and Lewis acis sites, the alkylation of toluene using benzyl alcohol or benzyl chloride was performed following a previously published procedure [14]; 100 mg of the catalyst (for benzyl alcohol) and 250 g (for benzyl chloride) were placed in a special pyrex tube and activated in a oven at 250~ for one hour. The tube containing the catalyst was cooled to the reaction temperature (50~ for benzyl chloride or 80~ for benzyl alcohol) and placed in a glycerol bath already at the reaction temperature. A pre-heated mixture made up of 20:1 molar ratio of toluene and the alkylating reagent was added to the catalyst with magnetic stilting. The reaction was carried out under a continuous flow of synthetic air. Reaction mixture samples were collected in vials every 30 minutes and analysed by gas chromatography. 3. RESULTS AND DISCUSSION The elemental compositions of the present AI-MMS materials are shown in Table 1. The bulk Si/A1 ratios of the samples indicate that Si and A1 are incorporated into the solid framework in proportions closely related to the synthesis gel composition. A significant observation worth pointing out is that A1-MMS40 and AI-MMS 10 are AI rich, i.e., a greater proportion of A1 in the synthesis gel is incorporated into the solid product compared to Si. This is a departure from our previous studies where we always obtained silica rich materials [9-13]. This is the first indication that the modified synthesis procedure used here, in which the dissolution of the AI source is optimised, does allow for greater A1 incorporation into the solid product. In our previous studies, the synthesis of A1-MMSX materials did not include the ahmainium isopropoxide dissolution step, i.e., the vigorous stilting of the A1 source in isopropanol at 70~ for 15 min was not performed. It is likely that the dissolution step enables a much higher proportion of the aluminium isopropoxide to dissolve thus forming AI species which readily interacted with the silica species after the addition of TEOS to form AIrich polymeric aluminosilicate species. Powder XRD pattems for the present AI-MMS samples are shown in Figure 1(a). The patterns are similar to those of comparable mesoporous materials [ 11-13,15], i.e., comprising of a single (100) peak. This is an indication that the present samples are as well ordered as any other primary amine templated mesoporous aluminosilicates. It therefore appears likely that the higher extent of A1 incorporation achieved here does not compromise structural integrity. The d spacing and textural properties of the A1-MMS materials are shown in Table 2. We note that the d spacing of each of the present samples is lower (by ca. 5%) than we have previously observed for equivalent (in terms of synthesis gel Si/A1 ratio) materials [11 ]. We attribute the apparently smaller lattice size to the higher extent of AI incorporation achieved here. A feature common to both the present set of samples and those from previous studies is that the d spacing reduces as the amount of A1 incorporated increases [9-13]; this emphasises the importance of A1 content in determining the lattice size. It is worth noting that the d spacings observed here are generally lower than those normally obtained for M41S type mesoporous materials [ 1-3].
145
Table 1. Elemental Composition, acid content and catalytic activity of super-microporous A1-MMS samples. Sample Si/A1 Acid content Cumene conversion (%) (mmole/g) 50 min 150 min A1-MMS40 39.0 0.36 35 28 A1A1-MMS40 22.8 0.57 53 47 AI-MMS20 22.0 0.56 47 41 A1A1-MMS20 14.9 0.75 59 54 A1-MMS10 9.0 0.73 59 51 A1A1-MMS 10 7.4 0.82 67 60 Table 2. Textural properties of super-microporous AI-MMS samples. Values in parenthesis micropore surface area and volume. Sample Basal (dl00) Surface Pore Spacing Area Volume (A) (m2/g) (cm3/g) A1-MMS40 32.4 1023 (488) 0.45 (0.18) A1A1-MMS40 32.0 643 (406) 0.33 (0.17) AI-MMS20 31.1 864 (497) 0.38 (0.19) A1AI-MMS20 30.2 562 (403) 0.28 (0.17) A1-MMS 10 30.5 684 (520) 0.31 (0.20) A1A1-MMS 10 29.8 358 (286) 0.24 (0.18) (a)
are Pore
Size 20.5 17.7 18.4 16.3 17.7 14.5
(b)
.m c-
t_
.m
E
0
2
4 2a/~
6
8
i
|
|
2
4
6
8
2~
Figure 1. Powder X-ray diffraction patterns of primary amine templated super-microporous aluminosilicates before (a) and after (b) post-synthesis grafting of A1.
146 The clearest indication that the greater AI incorporation attained here results in materials with super-microporous rather than mesoporous character is given by the textural parameters in Table 2. First we note that the surface area, pore volume and pore size obtained for the present samples are generally lower than previously observed for mesoporous A1MMS (AI-HMS) materials [ 11-15]. We have previously reported surface area of 1200, 1195 and 967 m2/g, and pore volume of 0.65, 0.52 and 0.49 cm3/g for mesoporous AI-MMS materials prepared (with dodecylamine as terriplate) at gel Si/A1 ratios of 40, 20 and 10 respectively [11]. The pore volume of the present samples is therefore at least 30% lower than that of analogous mesoporous materials [ 11]. A particular feature of the present samples is that they exhibit a high proportion of micropore surface area and volume as shown in Table 2. This is a significant finding because we have not previously observed any micropore surface area or volume in, for example, mesoporous AI-MMS40 and A1-MMS20 materials [ 11]. In the present samples the proportion of micropore surface area increases from 47% for AI-MMS40 to as high as 76% for A1-MMS 10 while the proportion of micropore volume rises from 40 to 65%. We attribute the high level of microporosity observed for the present A1-MMSX materials to the super-microporous nature of the pore channels they possess. The pore size of the materials (obtained using BJH analysis) is, as shown in Table 2, clearly in the supermicroporous range. This is also illustrated by the N2 sorption isotherms shown in Figure 2. The isotherms exhibit high adsorption at low (P/Po < 0.2) partial pressures which is characteristic of super-microporous materials. The isotherms do not exhibit the mesopore filling step (at P/Po > 0.2) normally observed for mesoporous materials. In Figure 2 we have, for comparison, also included sorption isotherms for equivalent (w.r.t. synthesis gel Si/A1 ratio) materials, which have been synthesised without the A1 dissolution step. Such materials
~, 400 ~
400
o~~ 300 i
300
~
200 J
i
1~ 100
"~
o
200 100
0.0
0.5
Partial pressure
1.0
(PIPo)
o
0.0
0.5
Partial pressure
1.0
(PIPo)
0.0
0.5
Partial pressure
1.0
(PIPo)
Figure 2. Nitrogen sorption isotherms of primary amine templated mesoporous aluminosilicates (top) and super-microporous aluminosilicates (middle), prepared at gel Si/A1 ratio of (a) 40, (b) 20, (c) 10. The bottom isotherms are for the super-microporous aluminosilicates after they were subjected to post-synthesis grafting of A1.
147 typically possess 15-20% less A1. As shown in Figure 2, the lower A1 content materials have larger pores and in some cases (top isotherm Figure 1(a)) exhibit a clearly defined mesoporefilling step. Post-synthesis grafting of A1 was found to increase the microporous character of the A1-MMS samples. The effect of Al-grafting on pore size and porosity is illustrated in Figure 2; the super-micropore filling step is shifted to lower partial pressures (lower pore size) after grafting. As shown in Table 2, the pore size of A1A1-MMS samples is lower than that of A1MMS materials by 2 to 3 A. This reduction in pore size is accompanied by a decrease in surface area and pore volume, which in turn leads to an increase in the proportion of micropore surface area and volume. Indeed sample A1AI-MMS 10 is virtually microporous, with a pore size of 14.5 A and a proportion of micropore surface area and volume above 75%. It is likely that the extra A1 is grafted onto the inner pore walls of the AI-MMSX materials thus reducing the pore size. This does not however affect the basal spacing (see Table 2) since the pore shrinkage occurs within existing pores. We note that structural ordering (as indicated by powder XRD - see Figure l(b)) is largely unaffected by the grafting process. Only modest reductions in the intensity of the basal peak are observed. We however do not think that this reduction in the intensity of the basal peak is due to degradation of structural integrity. It is more likely caused by changes in the scattering domain size (SDS), i.e., the SDS reduces during grafting. Indeed using scanning electron microscopy (SEM), we have observed that the particle size of A1A1-MMSX samples is smaller than that of the AIMMSX sample from which they are derived. This is illustrated in Figure 3 for A1-MMS20 and A1A1-MMS20 samples. It is noteworthy that although the particle size reduces, the spherical particle morphology is maintained after grafting. A uniform particle size is also retained after grafting. (a) A1-MMS20
(b) A1A1-MMS20
Figure 3. Representative scanning electron microscopy (SEM) micrographs of (a) A1-MMS20 and (b) A1A1-MMS20 illustrating the effect of post-synthesis Al-grafling on the particle size. Scale bar = 10 gm. In addition to tailoring the pore size, Al-grafiing also increases the acid content and catalytic activity as shown in Table 1. The increase in acid content after A1 grafting is greatest
148 for A1A1-MMS40 (-~ 60%) and lowest for AIAI-MMS 10 (- 12%). The introduction of extra AI clearly creates new acid sites. This is possible since the AI-MMS materials possess exposed and accessible silanol groups, which can act as anchoring points for the extra AI [ 16,17]. For extra acid sites to be generated, some of the extra A1 must be incorporated into the framework. We note that 27A1 MAS NMR spectroscopy indicated that the majority of AI in the A1A1-MMSX samples is in tetrahedral coordination. The proportion of octahedrafly coordinated (extra-framework) AI in A1A1-MMSX samples is however generally higher than that for corresponding AI-MMSX samples indicating that some of the extra AI is not incorporated into the framework. It is interesting to note that sample A1-MMS 10 which has the highest cation exchange capacity (CEC = 42 mEq/100g) takes up less 'extra AI' than AIMMS40 with a CEC of 12 mEq/100g. This implies that the take up of extra AI is not entirely an ion exchange process. Rather it appears that the extra AI is taken up chiefly via a grafting process that occurs on silanol groups [16,17]. This is consistent with our previous observation that the concentration of silanols in A1-MMS type materials decreases with A1 content [11]. It is therefore expected that A1-MMS40 would have more silanol groups (capable of anchoring greater amounts of extra A1) compared to AI-MMS10. Indeed under similar grafting conditions the pure silica material incorporates at least twice as much A1 as the A1-MMS samples. The solid acid catalytic activity of AI-MMS (AI-HMS) materials is a well studied topic. Here the discussion on catalytic activity is restricted to the differences between A1-MMS and AIAI-MMS materials. As shown in Table 1, all samples present considerable catalytic activity for the conversion of cumene. The percentage of cumene cracked (predominantly to benzene and propene) depends directly on the Si/A1 ratio and the acid content. Comparison of the activity at 50 and 150 min. indicates that the rate of deactivation is comparable for all samples. It is also clear that A1AI-MMS samples are more active than their corresponding AIMMS samples. The increase in activity, on grafting, is highest for A1-MMS40 and lowest for AI-MMS 10. The increase in activity for cumene conversion after grafting therefore mirrors the percentage (and absolute) increases in A1 content and acidity. Furthermore since the cumene conversion to benzene and propene occurs on Bronsted acid site, we may infer that there is an increase in the number of Bronsted acid sites after grafting. The catalytic activity of Bronsted and Lewis acid sites can be separately evaluated using the alkylation of toluene. Bronsted acid activity was tested using the alkylation of toluene with benzyl alcohol and Lewis activity was tested using the alkylation of toluene with benzyl chloride. In both cases 1,2 and 1,4 methyldiphenylmethane are the main products and the activity is pseudo-first-order rate for both reactions. In all cases Al-grafting was found to increase the extent of alkylation. In Figure 4, the effect of gratting extra AI is illustrated using sample A1-MMS20. The extent of alkylation over AIA1-MMS20, for both reactions, was found to be consistently higher at all reaction times. The variation of rate of alkylation with time suggests that Alkylation over A1A1-MMS20 may approach equilibrium quicker than happens for A1-MMS20. We note that similar trends were observed for A1-MMS40 and A1MMS10 and their grafted derivatives. The catalytic data in Figure 4 therefore shows that grafting of extra AI has beneficial effects not only for Bronsted acid catalysis but also for Lewis acid catalysed reactions.
149
30
(a)
(b)
25 o~ tO i,..
(D > c"
O (O
20 15 10
,
,
,
i
0 1 2 3 4 5 6
0 1 2 3 4 5 6
Time (hour)
Time (hour)
,
,
Figure 4. Conversion as a function of reaction time in the alkylation of toluene using (a) benzyl alcohol and (b) benzyl chloride on A1-MMS20 (dark symbols, 9 and o) and AIA1MMS20 (open symbols, [] and o). Primary amine templating of mesostructured aluminosilicates is known to provide solid acid catalysts whose activity is generally higher than that of materials prepared via quaternary ammonium ion templating [11,12,18]. The improved activity has been variously attributed to a number of factors including improved accessibility to acid sites, a unique pore structure and textural mesoporosity, which allow easy diffusion of molecules [11,12,15,18]. Recently, it has also been shown that the wormhole-like structure of primary amine templated aluminosilicates has 3-dimensional connectivity [19]. Three-dimensional connectivity is an important factor with respect to catalytic activity. This report therefore represents the first synthesis of super-microporous aluminosilicates with 3-dimensional connectivity. These super-microporous materials combine all the advantages of primary amine templated aluminosilicates and also offer the potential for size and shape selective catalysis of large substrates which is not possible for mesoporous materials. ACKNOWLEDGEMENTS EBG would like to thank CONICIT for the Venezuelan financial support. COT and ORS scholarships are also acknowledged. R.M. is grateful to the EPSRC for an Advanced Fellowship. REFERENCES
1. A. Corma, Chem. Rev., 97 (1997) 2373. 2. C. T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710.
150 3. 4. 5. 6. 7.
J.Y. Ying, C. P. Mehnert and M. S. Wong, Angew. Chem. Int. Ed., 38 (1999) 56. S.A. Bagshaw and A. R. Hayman, Chem. Commun., (2000) 533. X.S. Zhao, G. Q. Lu and X. Hu, Chem. Commun., (1999) 1391. T. Sun, M. S. Wong and J. Y. Ying, Chem. Commun., (2000) 2057. D.P. Serrano, J. Aguado, J. M. Escola and E. Garagorri, Chem. Commun., (2000) 2041. 8. E. Bastardo-Gonzalez, R. Mokaya and W. Jones, Chem. Commun., (2001) 1016. 9. R. Mokaya and W. Jones, Chem. Commun., (1996) 981. 10. R. Mokaya and W. Jones, Chem. Commun., (1996) 983. 11. R. Mokaya and W. Jones, J. Catal., 172 (1997) 211. 12. R. Mokaya and W. Jones, Catal. Lett., 49 (1997) 87. 13. R. Mokaya and W. Jones, J. Mater. Chem., 8 (1998) 2819. 14. H. H. P. Yui and D. R. Brown, Catal Lett., 56 (1998) 57. 15. W. Z. Zhang, T. R. Pauly and T. J. Pinnavaia, Chem. Mater., 9 (1997) 2491. 16. R. Mokaya and W. Jones, Phys. Chem. Chem. Phys., 1 (1999) 207. 17. R. Mokaya and W. Jones, J. Mater. Chem., 9 (1999) 555. 18. T. J. Pinnavaia and W. Z. Zhang, Stud. Surf. Sci. Catal., 117 (1998) 23. 19. J. Lee, S. Yoon, S. M. Oh, C. H. Shin and T. Hyeon, Adv. Mater., 12 (2000) 359.
Studies in Surface Scienceand Catalysis 141 A. Sayariand M. Jaroniec (Editors) 9 2002 ElsevierScienceB.V. All rightsreserved.
151
A 1 - M C M - 4 1 synthesis using Al-isopropoxide as A1 source R. Birjega, R. Ganea, C. Nenu, Gr. Pop and A. Jitianu ZECASIN, Spl.Independentei 202, PO-Box 12 304, 77206 Bucharest, Romania. Fax: 40 1 3125241, e-mail: zecasin@ com.pcnet.ro *Institute of Physical Chemistry "I.G.Murgulescu", Bucharest, Romania. 1. INTRODUCTION Since a new family of mesoporous materials designated as M41S was first introduced to the scientific community by the scientists from Mobil Corporation [1,2] a great deal of work was devoted to the possibility of isomorphous substitution of heteroatoms, especially aluminum, into the silica network, in order to modify the composition of the material. The aluminum substitution in silica MCM-41 is of particular interest, both for an academic or technological approach, as the expected acid properties and ion exchange capacity modifications, allowing the design of catalysts or catalyst support materials for further active species grafting. Numerous preparation strategies were described with a variety of chemical systems and different raw materials [3-10]. The synthesis of the ordered mesoporous materials implies a complex array of reactions in media where reactants organic and inorganic species and conditions can be continuously changed. In this work we focused on a series of A1-MCM-41 an aim to establish an appropriate Si/A1 atomic ratio domain of the reaction mixture to be used in relatively low concentration surfactant syntheses. The synthesis conditions were selected bearing in mind a possible application at large scale of such materials. The surfactant used was cetyltrimethylammonium bromide (C16TMABr). As silicon source a combination of alkali silicate, organic silicate and pure silica powder, was used. Aluminum isopropoxide, a monomeric alumina precursor was selected as alumina source. Janicke et al. [3] claimed that aluminum isopropoxide, as aluminum source is efficient in controlling Al-framework incorporation, while different results were reported by Luan et al. [7]. Janicke et al considered that syntheses employing aluminum isopropoxide yielded products required gentle heat treatment in an inert atmosphere of flowing nitrogen followed by calcination in flowing oxygen. However, we performed all the calcinations in air with low heating ramp l~
152 2. EXPERIMENTAL SECTION 2.1 Synthesis A series of mesoporous aluminosilicate A1-MCM-41 have been synthesized using cetyltrimethylammonium bromide (C16TMABr, Fluka) as surfactant. A1-MCM-41 syntheses of different Si/A1 mole ratios (5-120) at low surfactant concentration (CI6TMABr/SiO2 mole ratio= 0.15 ) using similar procedures to those reported [1-3] were performed. The nature of the silicon precursor is considered to be an essential factor for obtaining a high-quality MCM-41 mesoporous material. Although, it has been used as silicon source, various raw materials, the degree of condensation of the walls and the degree of pore ordering are influenced by a proper choice of the silicon precursor in connection with the synthesis conditions. Highly basic gels favor the lamellar phase, while weakly basic gels lead to the formation of amorphous silica. The alkalinity level of the synthesis gel plays an important role in the MCM-41 formation. Consequently, a combination of alkali silicate, organic silicate and pure silica powder is preferred to be used as a silicon source [4,5]. Therefore, we used a mixture of sodium silicate, tetramethylammonium silicate and fumed silica as an adequate silicon precursor for A1MCM-41 syntheses. Aluminum isopropoxide (Merck) was the aluminum source and tetramethylammonium hydroxide solution (25% TMAOH, Aldrich) was used as mineralizer. The aluminum-containing gels were prepared as follows: Firstly, a tetramethylammonium silicate solution (TMA/Si=0.5, 10% SiO2) was prepared by mixing appropriate amounts of 25% TMAOH solution and fumed silica (98% SiO2, Sigma). Then, the sodium silicate solution (27% SiO2, 9% Na20, Merck), water and fumed silica were added to the teramehylammonium silicate solution, under continuous stirring. Secondly, a 15% aqueous CI6TMABr solution was added to the above silicate mixture under vigorous stirring and a well-homogenized gel was obtained. Finally, an adequate amount of aluminum isopropoxide was added into the surfactant-silicate mixture. The mole chemical composition of the aluminosilicate gel was: SiO2:0.07Na20:0.085TMAOH:0.004-0.40A1203:0.15C16TMABr:60H20 A reference synthesis using only purely siliceous synthesis gel was prepared by the same procedure, without the addition of the aluminum source. After stirring for one hour at room temperature the synthesis gel having, a pH around 12 was loaded into a 500 ml Teflon-lined autoclave and heated at 100~ for 48 hours, under continuous stirring. After cooling to room temperature, the resulting product was repeatedly washed with distilled water until the pH reached 7.5, separated by filtration and dried in air, at room temperature. The surfactant was removed from the as-synthesized product by calcination in air (static conditions) with a heating rate of I~ from room temperature to 550~ and maintained at 550~ for 6 hours.
153 2.2 Characterization
The as-synthesis and calcinated samples were characterized by X-ray powder diffraction on a DRON-3 diffractometer using monochromated CuKa radiation. Diffractions patterns were recorded from 1~ to 30~ (20) with a resolution of 0.02~ and a count time of 20s at each point. The diffraction peaks were fitted assuming a Pearson-VII function for the peak profile. SiO2 a-quartz was used as internal standard as well as for the background extraction in the low angle region. The IR spectra were recorded between 1600 cm1 to 400 cm1 with a SPECORD M80 spectrophotometer using KBr pellets technique. The BET surface areas were measured by the N2 physisorption at 77K using a Grimm BET automatic surface analyzer. A preheating in a helium atmosphere at 200~ for 2 hours was performed in order to consider the percent of water in the calculation of the BET surface areas. The overall acidity of the samples was evaluated by a NH3-TPD. The procedure consists of: the preheated of the samples at 200~ for 2 hours in argon stream, the saturation of the surface with ammonia at 120~ in a mixture of ammonia-argon gas stream and the removal of the physically adsorbed ammonia. Finally, the temperature was linearly ramped up to 600~ and the total amount of desorbed ammonia was continuously trapped in sulfuric acid solution and quantified by titration with NaOH solution. For comparison, the acid content of the samples was also evaluated using a simple method of titration with a hydroxide solution, taking into account that one equivalent of base corresponds to one equivalent of proton (H§ associated to the framework aluminum sites [11,12]. 3. RESULTS AND DISCUSSION As figure 1 shows, except for the high aluminum content synthesis (Si/Al=l.25), the XRD patterns of the as-synthesized sample exhibit well -defined peaks of pseudohexagonal structure of MCM-41. The peaks are indexed in P6 symmetry with a lattice constant ao, actually the distance between the centers of two neighbor pores, calculated as ao=2dl00/~/3. Along with the pattern of an ordered channels disposition, the broad peak appearing between 20-25 ~ (20) usually assigned to an amorphous silica or silica-alumina ,is considered. Table 1 presents the structural data of the as-synthesized MCM-41 samples. o
A I/(A
I+ S i)
0.032 ".444
0
~ 2oC
uKa(*)
Figure 1. XRD pattems of as -synthesized MCM-41 content
samples with different aluminum
154 From the data presented in Table 1 one could notice the effect of aluminum incorporation into MCM-41 materials. For low contents of aluminum the diffraction intensity of the main peak is higher than that of the pure silica analogue suggesting a tendency of an improvement of the condensation of the silica structures in the presence of the aluminum. There is no a regular increases of the lattice constant ao with the aluminum content due probably, to the low aluminum amount and a high amount of silanol groups. For the last sample, the small ao value is explained by the formation of aluminum-rich dense phase, confirmed by SEM and BET measurements and therefore a low content aluminum MCM-41 is formed in this case. There is a linear relationship between the relative intensities of the 110 diffraction peak and the relative intensities of the 210 peak to the 200 peak. This result is in agreement with the model structure for MCM-41 proposed by Feuston & Higgins [13]. In the simulated patterns in accordance with the experimental patterns, the relative intensity of this peak decreases with increasing wall thickness. In the as -synthesis forms the presence of aluminum seems not to increase perceptive the wall thickness. One should also noticed that the full width at half maximum height of the 100 reflection FWHM increased with the aluminum content as a sign of a slight distortion of the long range order induce by aluminum incorporation. However, the A1-MCM-41 samples exhibit a slight decrease of the broadness of the 100 peak after calcination in contrast with the Si-MCM-41 analogue which 100 peak is broader after calcination. The Al-rich synthesis leading to a mixture phase composition thermally unstable is not included in this trend. A broad peak suggests also small particle size, confirms by SEM micrographs for the relative larger amounts of aluminum. Table 1. XRD data of as-synthesized MCM-41 samples Sam pie 1 2 3 4 5 6 7 8 9
A1 mole fraction 0 0.008 0.013 0.016 0.020 0.024 0.032 0.063 0.167 ,,,
ao (A) 51.14 50.97 51.77 50.61 51.31 51.44 49.72 51.26 47.92 ,,,,,
,,
MCM-41 I100 FWHM100Ill0 (a.u.) ( o) (a,u.) 8.32 0.25 0.88 7.65 0.28 0.46 9.32 0.26 0.68 7.32 0.28 0.72 7.00 0.28 0.75 7.76 0.27 0.52 6.08 0.30 0.66 5.67 0.32 0.25 4.61 0.25 0.79 ,,
,
Amorphous p e a k Ill0/I1001210/1200 d I FWHM (A) (a.u.) (o) 0.106 0 . 6 1 4.15 0.262 1.12 0.061 0.89 4.18 0.268 1.10 0.073 0.78 4.17 0.263 1.12 0.099 0.62 4.15 0.239 1.06 0.107 0 . 6 1 4.15 0.236 1.04 0.067 0.96 4.18 0.259 1.14 0.109 0.60 4.13 0.228 1.09 0.043 1.05 4.18 0.216 1.17 0.108 0.44 ,,,,
,
,
,
,
,,,,,,,,
,,,,,
,,
,
,
,,,,
It could be observed that the intensity of the 100 peak decreased with the intensity of the broad amorphous peak .It means that main contribution to the intensity of this peak is provided by the disordered material of the walls. As an intrinsic property of MCM-41 material is worth to give more attention to the analysis of this peak [14]. After the calcination procedure, the XRD diffraction pattems of the samples present the already reported behavior [1-7,5,15]: an enhancement of the peak intensities and a shrinking of the lattice as a result of surfactant removal and a subsequent condensation ofsilanol groups. Upon calcination a displacement towards higher angles
155 along with a decrease of the intensity of this maxim are observed. The result is to be connected with structural water removal. The structural data are collected in Table2. Table2. Structural data of calcinated MCM-41 samples Sample
1 2 3 4 5 6 7 8
A1 mole fraction 0 0.008 0.013 0.016 0.020 0.024 0.032 0.063
Lattice contraction (%) 7.16 5.80 9.06 6.69 7.99 6.85 6.86 9.60
I100eale/I100synt__FWHM100calc/FWHM100synt Weight loss (%) 2.432 1.089 48.74 2.568 0.908 49.15 2.629 0.926 49.60 2.384 0.976 48.55 2.611 0.980 48.00 2.428 1.009 47.56 2.253 1.000 46.44 2.317 0.933 44.84
Apart from sample 9, with high aluminum content (A1 mole fraction=0.167), which proves to be thermally unstable, all the samples exhibit well-defined typical MCM41 XRD pattems. The good quality of the materials is pointed out also by the high total weight loss and also by the relatively low contraction lattice. It was already mentioned that for the Al-containing MCM-41 samples calcination improves the restructuring process of the walls reflected by a sharper 100 diffraction peak in comparison with the assynthesis forms. The result could be attributed to an initial lower silanol groups amount. The 27A1 MAS NMR spectrum of as-calcined sample 7 (figure 2) proves clearly that almost all the A1 ( 94 %) are tetrahedrally coordinated ( 53.8 ppm) . The octahedral aluminum NMR signal (0 ppm) are influenced also a by the degree the sample hydration[ 16]. .
.
m
.
m
.
.
.,,=
I
-400
-2;o
"
o'
20'0
"
4o'o
ppm
Figure 2. The 27A1MAS NMR spectrum of calcinated sample with an A1 mole fraction = 0.032
156 The IR spectra of the as-calcinated samples are similar with those reported for siliceous MCM-41 [1] with four adsorption bands at 1080 cml , 800 cm1, 960 cm1 and 450-470 cm1. The T-O-T band at 1080 cm"1 usually indicating the MCM-41 formation presents a slight shift to lower wavenumbers as the A1 content increases. The 960 cm1 maximum assigned to Si-OH groups became less well-defined also with the aluminum amount increment. For the highest A1 content sample this maximum is entirely overlapped by the 1080 cm1 one (figure 3). ~ A I I ( A I+ S i) 0.032 c In E
. o
/..~
"
o12,
~ o
40'0
60'0
8(~0
10~)0
wavenum
12100 ber
14=00
16~)0
18=00
20'00
( c r n "')
Figure 3. IR-spectra of two calcinated A1-MCM-41 samples The measurements of the acidityare presented in Table 3. Table 3. The acidity measurements Sample
Ai mole fraction
1 2 3 4 5 6 7 8 9
0 0.008 0.013 0.016 0.020 0.024 0.032 0.063 0.167
,,
,,
,
,,
,
,
Acid measurements ............ NH3-TPD (mmol/g) NaOH titr~ion(mmol/g) 0.1100 0.0843 0.2000 0.1849 0.4383 0.1874 0.2960 0.1925 0.2800 0.2000 0.2850 0.2025 0.2992 0.2575 0.5038 0.3000 0.6042 0.1875 ,,
,,,,
,,,,
,,,,,,,
,
,,,,,
,,,
The above data show a difference between both methods of acidity evaluation. The NaOH titration could be more accurate correlated with framework A1, and consequently with Broensted acidity and therefore it displays a rather good linear relationship with the A1 content. The NH3-TPD measurements imply both Broensted and Lewis acid sites and therefore the overall acidity is higher. There is no obvious linearity of the ammonia acidity with the A1 content probably due to different silanol groups amount. The rich-A1 sample
157 which is a mixture of MCM-41 and a dense amorphous phase exhibits, as expected, a low NaOH acidity due to framework A1 and higher total acidity (ammonia-TPD) provided by the dense phase. The SEM images and the BET surface areas (figure 4) proved for the formation of high quality ordered mesoporous materials up to an A1 mole fraction of 0.063. The rich A1 amount samples exhibit upon calcination, a poorly resolved XRD pattern, a less wellresolved IR spectrum, a SEM image with large portions of non-porous material and a low BET surface area.
A1/(AI+Si) = 0 ....~ !~'~,~~!ii~iI
BET=1123 m2/g
A1/(Al+Si):0.032 BET=1090 m2/g
A1/(AI+Si):0.167 BET = 332 m2/g
Figure 4. SEM micrographs of representative MCM-41 samples
158 In conclusion, our studies emphasize that it can be obtain a good-quality A1-MCM41 material, with well-resolved XRD patterns, high BET surface areas and acid properties in an range of AI mole fraction (A1/(AI+Si)) up to 0.063. It seems also that the presence of low amounts of A1 in the framework prevents 'the deterioration of the long-range structural order as in the case of siliceous MCM-41 occurred [17].
3. ACKNOWLEDGEMNTS We are grateful to Dr. Teresa Blasco ( ITQ, Valencia) for the record.
27A1MAS NMR spectrum
REFERENCES
1. J.S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T. -W. Chu, D. H. Olson, E. W. Sheppard, S. B. McCullen, J. B. Higgins, J. L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. 2. K.T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli, U. S. Pat., 5,098,684 (1992). 3. M. Janicke, D. Kumar, G. D. Stucky, B. T. Chmelka, Stud. Surf. Sci. Catal., 84 (1994) 243. 4. F. Schfith, Ber. Bunsenges Phys. Chem., 99 (1995) 1306. 5. C.T. Cheng, D. H. Park, J. Kinowski, J. Chem. Soc. Faraday Trans., 93 (1997) 193. 6. R. Schmidt, D. Akporiaye, M. Stk6cker, O. H. Ellestad, J. Chem. Soc., Chem. Commun., (1994) 1493 7. Z. Luan, C. -F. Cheng, W. Zhou, J. Klinowski, J. Phys. Chem., 99 (1995) 1018. 8. K.R. Kloestra, H. W. Zandergen, H. van Bekkum, Catal.Lett., 33 (1995)157. 9. H. Kosslick, G. Lischke, B. Parlitz, W. Storek, R. Frike, Applied Catalysis A: General, 184 (1999) 243. 10. W. B6hlmann, D. Michel, Stud. Surf. Sci. Catal., 135 (2001), 06p 17. 11. R. Mokaya, W. Jones, J. Catal., 172 (1997) 211. 12. R. Mokaya, W. Jones, J. Mater. Chem., 9 (1999), 533. 13. B. P. Feuston, J. B. Higgins, J. Phys. Chem., 98 (1994) 4459. 14. M. Ookawa, Y. Yogoro, T. Yamaguchi, K. Kawamura, Stud. Surf. Sci. Catal., 135 (2001) 06002. 15. M. T. Keene, R. D. M. Gougen, R. Denoyel, R. K. Harris, J. Rouquerol, P. L. Llewellyn, J. Mater. Chem., 9 (1999) 2843. 16. J. M. Kim, J. H. Kwak, S. Jun, R. Ryoo, J. Phys. Chem., 99 (1999) 16742. 17. R. Ryoo, J. M. Kim, J. Chem. Soc., Chem. Commun., (1995) 711.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
159
M e s o p o r o u s aluminosilicates from coal fly ash P. Kumar*, N. Mal, Y. Oumi~, T.
S a n o 1 and
K. Yamana
Ceramic Section of Chemistry & Food Department, Industrial Research Institute of Ishikawa, Kanazawa, Ishikawa 920-0223, Japan. E-mail:
[email protected] 1School of Materials Science, Japan Advanced Institute of Science & Technology, Tatsunokuchi, Ishikawa 923-1292, Japan
For the first time supematant of the coal fly ash has been used to prepare aluminum containing MCM-48. It was found that most of the Si and A1 components in the fly ash could be effectively transformed into MCM-48 when a surfactant mixture containing cationic cetyltetramethylammonium bromide, CTMABr and tetraoxyethylene dodecyl ether, C12(EO)4 is used as template. It has been observed that the fusion plays an important role in enhancing the hydrothermal condition for synthesis of these mesoporous materials. High concentration of Na ions present in the supernatant of fused fly ash is found to be not critical in the formation of A1-MCM-48 when prepared under controlled pH condition. 1. INTRODUCTION Although there are many articles concerning synthesis of mesoporous materials [1-2] most of them have been severely biased to MCM-41 [3-4]. The bias may be attributed largely to the fact that the synthesis of MCM-48 required very specific synthesis conditions [5]. MCM-48 (cubic, space group Ia3d) with its highly branched and interwoven threedimensional networks of the mesopore channels are believed to be much more resistant to pore blockage while being used as absorbents and catalyst supports than the onedimensional channel of a hexagonal MCM-41 [1,6]. Presently however, both the economic and environmental costs for large-scale manufacture of these materials are high due to the cost and toxicities of both templates and preferred silica source. A variety of silica sources are generally used to prepare these materials including fumed silica and silicon tetraethoxide. The industrial manufacture of mesoporous materials is likely to be economically prohibitive if silicon alkoxides and fumed silica in particular are selected. Coal combustion in the world accounts for approximately 37% of the total electricity production and in turn, results in the production of a huge amount of fly ash as waste material [7]. Nearly 600 million metric tons of fly ash are produced annually in the world, with the global recycling rate being only 15% [8]. Since the major chemical compounds contained in fly ash are SiO2 and A1203 (60-70 wt% and 16-20 wt%, respectively), resource recovery is one of the most important issues of waste management at present [9-
160 11 ]. Very recently we have reported our preliminary investigation on the synthesis of A1MCM-41 and SBA-15 type of materials and their characterization [12]. In this paper we report the studies carried out on the hydrothermal synthesis condition of the aluminum containing MCM-48 type materials using coal fly ash as a silicon and aluminum source and their characterization. Synthesis of both MCM-41 and MCM-48 is related in the sense that they can be prepared under identical hydrothermal condition subject to the type and concentration of surfactant used [ 1]. In addition to that various synthesis routes to MCM-48 were developed in order to overcome the synthesis shortcomings [ 13]. These synthesis results showed that the crystallinity of the MCM-48 went through an optimum as a function of time. The MCM-48 products were obtained as an intermediate between transformations from a hexagonal or disordered surfactant-silica mesophase to a more stable lamellar mesophase [14]. One report [15] suggested that the transformation of the MCM-48 mesophase to lamellar can be quenched by adjusting the pH of the reaction mixture. Another report [ 16] claimed that the mixed surfactant approach resulted into high quality MCM-48 as an energetically favored mesophase. Finally, it has been reported that the use of gemini surfactants induce the formation of cubic structure even using fumed silica as silicon source [17]. All these studies indicate that the formation of MCM-48 type materials is possible under certain synthesis conditions. Our aim in this study is to prepare MCM-48 type materials so we focus on three factors, a) single surfactant concentration, b) mixed surfactant concentration and c) intermediate pH adjustment. 2.
EXPERIMENTAL
2.1.
Materials Coal fly ash used in this study was obtained from Nanao-Ota power plant, Hokuriku and used as obtained. The chemical composition of fly ash revealed apart from the main constituents such as silica (67.5%) and alumina (18.7%), the other impurities such as Fe203, CaO, MgO, 1(20, TiO2, Cr203, P205 Na20, K20 and SO3 with 3.6%, 2.0%, 0.7%, 0.9%, 0.8%, 0.9%, 0.3%, 0.2%, 0.4%, 0.7%, respectively. The specific surface area (BET) and cation exchange capacity (CEC) of the coal fly ash were found to be 4.5 mE/g and 0.8 meq/100g, respectively. 2.2. Synthesis of AI-MCM-41 and AI-MCM-48 The silica and aluminum source was the supernatant from fused fly ash powder [ 18]. The concentrations of Si, A1 and Na in supernatant measured by atomic adsorption spectroscopy (Perkin Elmer AS-800) are 11000, 380 and 35000 ppm, respectively. The detail synthesis procedure for MCM-41 was followed from our previous study [12]. MCM48 materials in this study were synthesized using both single surfactant and a surfactant mixture. While CTMABr was used as a single surfactant, the mixture was prepared by using CTMABr and C12(EO)4 (Aldrich). All batches were prepared using a synthesis gel with the following molar composition: CTMABr/ C12(EO)4/H20/Si = 0.35-0.55/0.150.25/100/1. The obtained gel was stirred for thirty min., the synthesis mixture was placed in a Teflon lined stainless steal autoclave and heated at 373 K for 4 days under static condition. Intermittently, the reaction mixtures were cooled to room temperature after one day at 373 K and subsequently added with acetic acid to adjust the pH at 10.2. The MCM48 product was finally filtered after an additional heating at 373 K for another 3 days. To
161 remove the surfactant, the as synthesized sample was calcined in air under static conditions at 813 K for 6 hours, with a linear temperature ramp of 0.5K / min and two plateaus of 60 minutes each at 423 and 623 K. For a comparison an aluminum containing MCM-41 and MCM-48 were prepared following the procedure as reported in the literature [1, 13]. All the materials obtained were further calcined as explained above.
2.3. Analysis and Characterization Powder X-ray diffraction (XRD) patterns were measured using CuK~ radiation by using MAX18X. cE The chemical composition was analyzed with Li]2B404 method by using X-ray fluorescence (XRF) technique (Philips PW2400), BET surface area by N2adsorption at liquid nitrogen temperature (Belsorp 28SA) and morphology by scanning electron microscopy (SEM) using Hitachi S-4100. Transmission electron microscope (TEM) image was obtained by using JEOL 2010. FT-IR spectra of the self supporting wafers were measured by JEOL JIR-7000. TG-DTA analysis was performed using Rigaku TG-8120. Solid-state nuclear magnetic resonance resonance 29 Si and 27A1 NMR spectra were obtained on a Varian VXP-400. 3. RESULTS AND DISCUSSION Because larger amounts of Si and A1 species can be dissolved by fusion method, we adopted fusion approach in this study. Figure 1 summarizes the XRD patterns of the fly ash (a) and the fused fly ash (b) at 823 K. It can be seen that the major crystalline phases present in the fly ash are quartz, mullite and aluminosilicate glass, which are present as the amorphous phase. On the other hand, a ! i m ; w w i large amount of sodium silicate exists in b the fused fly ash (Figure l b), which implies Ss that fusion is effective in extracting silicon from quartz. Most of the quartz species have reacted with the NaOH and resulted s s s into the disappearance of the respective s s s~Ms peaks in fly ash. SsS s iLlij,~slls sS Ss I ~' M S S S Figure 2 shows the XRD patterns of .,.., different MCM phases of calcined samples Q a prepared under different surfactant / silica ratio. It can be seen that low concentration of surfactant (CTMABr) results into MCM41 type materials as suggested from the Q XRD pattern (Figure 2a) clearly displaying at least four reflections that are consistent M MMM M O Q with indexing to a hexagonal cell, typical of an MCM-41 product. The observation 10 20 30 40 50 60 70 of three higher angle reflections other than 20 (degree) the d]00 indicates that the product is likely Figure 1. X-ray diffraction profiles of the to possess the symmetrical hexagonal pore fly ash (a) and the fused fly ash (b) at 823 structure typical of MCM-41. A further K. M = mullite, Q = quartz, and S = increase in surfactant concentration sodium silicate resulted into mesophases, poor in
162
Table 1 Physical properties of the raw material and the calcined mesoporous materials Sample Surf i Surf2 SBET/ Si/A1 Pore d 100 d 211 ao 3 /SiO2 /SiO2 m 2 g-i volume /nm /nm /nm
Pore size 4 /nm
/ c m 3 ~-1
Fly ash A1-MCM-41 (a) A1-MCM-41 (b)
0.20 0.35
-
4.5 842 738
2.9 13.8 18.5
. 0.75 0.57
A1-MCM-41 (c)
0.55
-
731
65.0
0.57
A1-MCM-48 (d)
0.55
0.15
639
62.3
A1-MCM-48 (e)
0.55
0.18
848
59.4
1 2 3 4
.
. 4.24 3.56
. -
4.9 4.1
3.2 2.9
3.56
-
4.1
2.7
0.55
-
3.17
7.8
2.5
0.82
-
3.04
7.4
3.0
cetyltrimethyl ammonium bromide tetraoxyethylene dodecyl ether unit cell parameter, using 2d100/~ for MCM-41 and d211 q5 for MCM-48 Dollimore-Heal method
hexagonal structural order as indicated from the gradual disappearance of diffraction peaks assigned to (110), (200) and (210) reflections (Figure 2b, 2c). The surfactant / silica ratio higher than 0.55 resulted into to a featureless XRD pattern (not shown). By increasing the concentration of CTMABr in the synthesis gel, a phase transitions from hexagonal to lamellar passing through an intermediate state of cubic structure is reported [1-4]. But using the supernatant as silica source it was not observed, in other words MCM-48 formation was not facilitated under the synthesis condition using CTMABr 211 alone. Figure 2d and 2e shows the 5 XRD patterns of the surfactant-silica mesophase obtained from the starting mixtures of CTMABr/ C12(EO)4 = 0.55/0.15 and 0.55/0.18, respectively. _= It can be seen the presence of neutral surfactant has resulted into mesophase, identical to the cubic MCM-48. We observed that the optimum condition ~ b for MCM-48 using supernatant as 110 silica source was 0.55/0.18 as it showed the sharpest XRD patterns. 4 6 8 Table 1 summarizes characteristics of 20 / degree the calcined mesoporous materials Figure 2. XRD profiles of the different obtained. calcined M C M type materials. CTMABr/SiOE 9a - 0.22, b - 0.35, c, d and e -- 0.55; C12(EO)4/SIO2: d - 0.15 and e - 0.18 9
!
9
!
,
4•
>,
e-
i
|
--
163 From this synthesis experiment the XRD pattern in Figure 2e, a highly ordered MCM-48, without any trace of lamellar phase peaks was recovered. The high ordered array of these materials could be inferred from the presence of a well def'med set of diffraction peaks between 3 ~ and 6~ the XRD patterns assigned to the (211), (220), (321), (420), (422) and (431). Gel representing higher than 0.18 of C12(EO)4 resulted either into unidentified mesophase or without any XRD pattern. The (211) reflection is found at approximately 3.6 nm for all the as-synthesized samples. This correspond to a unit cell size of 8.7 nm. For the calcined samples the same reflection occurs at-3.1 nm, which gives a unit cell length o f - 7 . 5 nm. Hence, as should be expected, there has been a shrinkage of the unit cell ( - 1 3 % ) during calcinations which probably Figure 3. N2 adsorptionis due to silanol condensation. This magnitude desorption isotherms of different of unit cell shrinkage was in the range of values samples (c, d and e), prepared normally reported in the literature using other under different conditions. silicon source, that are in the 5-15% range [1417]. The same tendency is observed for the (220) reflection suggesting that the supernatnt of coal fly ash could be used as a source material. The N2 adsorption-desorption isotherms of different samples (c, d and e) are shown in Figure 3. It corresponds to a reversible type IV isotherm which are characteristic for mesoporous materials. An inflection point is observed at relative pressures between 0.25 and 0.3. This corresponds to the filling of the mesopores, and the sharp increase in the adsorbed volume indicates a uniform pore-size distribution. It can be seen (Table 1) how the presence of neutral surfactant facilitates the formation of MCM-48. The presence of a small hysteresis loop in sample c, indicates the formation of lamellar phase which is very similar to the studies that has been reported at high surfactant/ silica ratio [19]. Figure 4 shows SEM images of the mesoporous materials prepared from the Figure 4. SEM images of fly ash and samples c ,d and e supernatant and the original fly prepared from supernatant of coal fly ash.
164 ash. Morphologically, the fly ash consists essentially of aluminosilicate glass spherules that disintegrate during fusion treatment and are converted into amorphous sodium silicate and sodium aluminosilicate. The SEM images of mesoporous materials are generally Figure 5. SEM images A1-MCM-41 (1) and A1-MCM-48 found in a range of (2) using pure chemicals. spherical top, ribbon, torous shape d particles [20]. In the present case, the particles of the materials obtained have a spherical habit at around less than 1 lxm although some agglomerates are also visible (sample c). The presence of C12(EO)4 as neutral surfactant resulted into more uniform spheres (sample d and e, respectively). In Figure 5 we have compared the SEM images of MCM-41 and MCM-48 by using pure chemicals such as TEOS and Al(NO3)3 as silicon and aluminum sources, respectively. The major particles of MCM-41 (sample 1) are constructed from elementary units that have ribbon-like habits. Formation of such ribbon-like particles are reported for MCM-41 when prepared under aged condition [21]. MCM-48 (sample 2) exhibited spherical raspberry-like pattern. Since both these samples are prepared from reaction mixtures differing in the surfactant / SiO2 ratio and content of water, this substantial difference in particle morphology are not unexpected. TEM images of micro-sectioned samples (Figure 6) also showed well ordered hexagonal arrays of mesoporous channel (sample a) and pores arranged on the cubic plane (sample e) confirming that the materials indeed possess the pore system symmetries that were inferred from the X-ray patterns and N2 isotherms. A mixed surfactant approach has been reported in the literature for the preparation of mesoporous materials [19]. In many cases, two different surfactants are completely miscible and form liquid crystalline miceller mesophase cooperatively. The structure in the micelle packing in the liquid crystalline mesophases may be determined by various effects such as their head to tail packing parameters, electrostatic interaction and hydrogen bonding between the head groups of the two different kinds of surfactant molecules [22]. This phase behavior becomes more complicated when silica and alumina sources are present in the Figure 6. TEM image of A1-MCMform of supernatant of coal fly ash. Supernatant is a highly alkaline solution of silicate and aluminate 41 (sample, a)and A1-MCM-48 (anions) and are strongly attracted by electrostatic (sample, e).
165 interaction surrounding the head groups of the CTMABr, which may lead to the high concentration of the anions on the surface of the surfactant micelles. The neutral surfactant has no strong interaction with the anions, and consequently its incorporation to the micelles will bring a dilution of the anions at the surface. This ~9 low surface concentration may further lead to a certain contraction of the micellar surface resulting in a phase transition from hexagonal to cubic. At this stage we are not advancing any explanation about the complexities of phase behavior of the fly ash supematant-surfactant mesostructures in the 10 5 0 aqueous solution, however we believe that ppm C12(EO)4 acts more as a diluents and based on our Figure 7. 27A1-MAS-NMR observation facilitated the formation of MCM-48 structure. spectra for fly ash and calcined Another factor that affected the formation A1-MCM-41 (sample a) prepared of cubic phase was the pH of the supematant- from supematant of fused fly ash surfactant mesostructure. Generally, a high pH solution. * Denotes the spinning condition is a major driving force for the side bands. transformation to lamellar [23]. In our case the pH adjustment to 10.2 during the synthesis arrested this transformation and also helped to improve the product yields. This is agreement with the report where the pH adjustment was mentioned as a means for quenching the transformation of the MCM-48 mesophase to lamellar [16]. We note that the BET surface area and pore volumes of the samples (Table 1) prepared in this work are slightly lower than those that may be obtained from more reactive silica sources. The values obtained are nevertheless similar to those reported in the literature and indicate high overall total porosity. Based on these observations, the possibility to use the dissolved silica and aluminum present in the supematant of fused fly ash as a precursor for the synthesis of MCM-48 are fairly good. But use of the high Si containing fly ash would be a better choice. One of the most important features of our study using coal fly ash is the aluminum incorporation into the framework of the synthesized materials [12, 18]. The information about the chemical state of A1 in the materials obtained using 27A1 MAS-NMR spectra of the original coal fly ash (a) and calcined A1-MCM-41 (b) were measured (Fig. 7). Fly ash did not show any peak, indicating the lack of any tetrahedrally (Td) coordinated framework aluminum. But a very strong single peak assigned to the Td framework aluminum at ca 54 ppm was observed for the sample prepared from fly ash without any Oh non-framework (0 ppm) aluminum. Even at such high aluminum concentration (Si/A1 = 13.8), absolutely no Oh peak was observed. This provides a direct evidence of A1 incorporation in the MCM-41 framework. Similarly, in the case of A1-MCM-48 (sample d and e) Td aluminum (spectra not shown) were observed though the presence of high concentration of surfactants has a dramatic effect on the aluminum incorporation as revealed from 27A1 MAS-NMR studies. ,
I
,
i
,
,
I
,
I
i
i
l
!
|
!
|
166 4. CONCLUSIONS In summary, it is shown that the supematant of coal fly ash can be used as a raw material for the synthesis of aluminum containing MCM-48. The use of surfactant mixture between cationic hexadecyl trimethylammonium surfactants and neutral tetraoxyethylene dodecyl ether surfactants has greatly facilitated the synthesis of MCM-48 performed under controlled pH condition. A high aluminum incorporation in tetrahedral position is revealed in the mesoporous materials which may be useful for certain catalytic applications. The experimental data produced here suggest that the coal fly ash could be a suitable source of silicon / aluminum with a low economy and environmentally friendly reagent for the preparation of well ordered mesoporous materials. REFERENCES
1. C.T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710. 2. S. Inagaki, Y. Fukushima and K. Kuroda, J. Chem. Soc., Chem. Commun., 1993, 680. 3. A. Corma, Chem. Rev., 97 (1997) 2373. 4. A. Sayari, Y. Yang, M. Kruk and M. Jaroniec, J. Phys. Chem. B, 103 (1999) 3651. 5. J.M. Kim, S. K. Kim and R. Ryoo, J. Chem. Soc., Chem. Commun., (1998) 259. 6. C.L. Landry, S. H. Tolbert, K. W. Gallis, A. M. Monnier, G. D. Stucky, P. Norby and J. C. Hanson, Chem. Mater., 12 (2001) 1600. 7. C. Zevenbergen, J. P. Bradley, L. P. V. Reeuwijk, A. K. Shyam, O. Hjelmar and R. N. J. Comans, Environ. Sci. Technol., 33 (1999) 3405. 8. G. Belardi, S. Massimilla and L. Piga, Resource, Conservation and Recycling, 24 (1998) 167. 9. A. Singer and V. Berkgaut, Environ. Sci. Technol., 29 (1995) 1748. 10. S. Rayalu, N. K. Labhasetwar and P. Khanna, U.S. Patent No. 6027708 (22 February 2000). 11. N. Shigemoto, S. Sugiyama, H. Hayashi and K. Miyaura, J. Mater. Sci., 30 (1995) 5777. 12. P. Kumar, N. K. Mal, Y. Oumi, K. Yamana, and T. Sano, J. Mater. Chem., 11 (2001) 3279. 13. M. L. Pena, Q. Kan, A. Corma and F. Rey, Microporous Mesoporous Mater., 44-45 (2001) 267. 14. A. Corma, Q. Kan and F. Rey, J. Chem. Soc., Chem. Commun., (1998) 579. 15. J. Xu, Z. Luan, H. He, W. Zhou and L. Kevan, Chem. Mater., 10 (1998) 3690. 16. R. Ryoo, S. H. Joo and J. M. Kim, J. Phys. Chem. B, 103 (1999) 7435. 17. P. Van Der Voort, M. Mathieu, F. Mees and E. F. Vansant, J. Phys. Chem. B, 102 (1998) 8847. 18. P. Kumar, Y. Oumi, K. Yamana and T. Sano, J. Ceram. Soc. Japan, 109 (2001) 968. 19. G. Oye, J. Sjoblom and M. Stocker, Microporous Mesoporous Mater., 27 (1999) 171. 20. K. Schumacher, M. Grun and K. K. Unger, Microporous Mesoporous Mater., 27 (1999) 171. 21. M. Grun, K. L. Unger, A. Matsumoto and K. Tsutsumi, Microporous Mesoporous Mater., 27 (1999) 207. 22. J. L. Palous, M. Turmine and P. Letellier, J. Phys. Chem. B, 102 (1998) 5886. 23. R. Ryoo and J. M. Kim, J. Chem. Soc., Chem. Commun., (1995) 711.
Studies in Surface Science and Catalysis 141 A. Sayariand M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rights reserved.
167
N e w route for synthesis o f highly ordered mesoporous silica with very high titanium content Xiang-Hai Tang*, Xin Wen, Shi-Wei Sun and Hai-Yan Jiang College of Chemistry, Nankai University, Tianjin 300071, P. R. China
Meso-structured titanosilicates with variable amounts of titanium have been hydrothermally synthesized under static conditions via a new route. By a separate hydrolysis procedure during gel preparation, this approach effectively prevents titanium ions from formation of indissoluble titanium species in the mixture at very high titanium content. The physicochemical properties of these materials were characterized by means of XRD, FT-IR, UV-Vis DRS and catalytic oxidation of 4-methylphenol with dilute hydroperoxide. In contrast to literature reports, this novel method can lead to mesoporous titanosilicates with a highly ordered MCM-41 hexagonal phase even in a gel with n(Yi)/n(Si) up to 1/4 and a relatively low template content. It reveals that these materials are chemically homogeneous. During crystallization, titanium ions were partially incorporated into the MCM-41 framework. The addition of TBAOH resulted in a more cross-linked and ordered wall structure.
1.
INTRODUCTION
The synthesis and characterization of hetero-atom containing molecular sieves have been a hotspot in the field of zeolite synthesis since the last two decades [ 1-5]. These materials are the most promising candidate catalysts for the environmentally benign industrial processes. Among them titanium-containing molecular sieves (e.g., TS-1, TS-2 and Ti-beta) have attracted considerable attention. However, their catalytic performance in reactions involving in bulky molecules is greatly limited due to the micropore nature, as their pore size is usually less than 2 nm. Fortunately, the pore diameter of solid materials with regular voids has been largely expanded since the discovery of M41S family materials. Up to now, mesoporous titanosilicates such as Ti-MCM-41 [6], Ti-HMS [7] and Ti-MCM-48 [8] have been successfully synthesized, but titanium content in these solids is usually very low. More recently, E1 Haskouri et al. [9] used a complexing polyalcohol (2,2,2-nitrile-triethanol) as a hydrolysis retarding agent for Yi species and reported that meso-structured titanosilicates could be prepared from a gel of n(Yi)/n(Si) up to 1/4. However, the framework of these materials was lack of long-range order, the BET surface area of the product with the highest n(Ti)/n(Si) of 1/1.9 in solid was merely 595 m2/g. It seems that these materials are analogues * To whom correspondence should be addressed. Email:
[email protected].
168 to Ti-HMS, and most of the titanium atoms locate outside the framework, which are lack of oxidation activity. Generally, the catalytic performance of mesoporous titanosilicate in selective oxidation reactions is dependent on the framework titanium and its amount. Hence it is of importance to develop new approaches for the preparation of high quality mesoporous titanosilicate. Here we demonstrate the synthesis and characterization of high titanium content MCM-41 titanosilicates with a highly ordered hexagonal phase. By our new approach high quality products could be prepared from a gel with n(Ti)/n(Si) up to 1/4 and a relatively low template content.
2.
MATERIALS AND METHODS
2.1.
Materials Tetraethyl orthosilicate (TEOS) and tetrabutyl orthotitanate (TBOT) were employed as silicon and titanium sources, respectively. Cetyltrimethylammonium bromide (CTABr) was used as template. Both liquid ammonia and tetrabutylammonium hydroxide (TBAOH) were used as hydrolysis agents. Firstly, TEOS, liquid ammonia and distilled water were mixed to prepare solution A, while TBOT was dropwise added to a mixture of TBAOH, ethanol and distilled water to prepare solution B. The two solutions were vigorously stirred in closed vessels respectively at ambient temperature till the solutions became homogeneous and transparent. Secondly, a gel was prepared by mixing solutions A and B, then the gel was boiled to evaporate alcohols and part of water. Finally, the gel was slowly added to a solution of CTABr, liquid ammonia and distilled water, and further stirred at ambient conditions for 3 h to obtain a mixture with a molar composition of (1-x)SiO2:xTiOz:yCTABr:O.3yTBAOH: mNH3:zH20 (where x=0-~0.2, y=0.1~0.7, z=100--520, m=6~l 1). The resultant was sealed in a PTFE-lined stainless steel autoclave and heated at 383 K for 72 h. The as-synthesized product was separated by centrifugation at 9000 rpm, washed twice with distilled water and later freeze-dried overnight to remove water from the solid product. To obtain the template free sample, the as-synthesized product was heated in air from ambient temperature to 823K at 7 K/min, kept for 4h, then raised temperature to 923K at 5 K/min and kept for lh. 2.2.
Characterization Powder X-ray diffraction (XRD) patterns were obtained in the 20 range 1-10 ~ with a Rigaku D/MAX 7A diffractometer using the Cu Ka radiation operated at 40 kV and 40 mA. FT-IR study was performed using a Bruker Vector-22 with a resolution of 4 cm ~ and 30 scans. The KBr technique with a sample to KBr weight ratio of 1"150 was used. UV-vis diffuse reflectance spectra (UV-vis DRS) were measured with a Shimadzu UV-240 spectrophotometer. Spectra were recorded in the 190-800 nm wavelength range against a MCM-41 standard. The catalytic activity of the calcined sample was tested by selective oxidation of 4methylphenol with dilute hydroperoxide. The reaction products were analyzed with a Hewlett-Packard HP G 1800A GC-MS instrument.
3. 3.1.
RESULTS AND DISCUSSION Material synthesis
169 Table 1 summarizes the gel molar compositions for preparation of various samples. Generally, hydrothermal syntheses of microporous zeolites and mesoporous materials are carried out in alkaline media. Unfortunately, most transition metal ions tend to hydrolyze and form insoluble species like metal hydroxides even in a neutral solution. To overcome that disadvantage and to increase the efficiency of metal source in the synthesis, it is essential to develop a new method to prevent the metal source from the formation of insoluble species. TBAOH, a strong base and an ionic surfactant, is commonly used as a structure-directing agent in zeolite synthesis. The hydrolysis of TBOT in a TBAOH-ethanol-H20 solution resulted in a mixture of soluble titanium species and effectively prevented or suppressed the formation of Ti(OH)4 and TiO(OH)2. Indeed, no visible precipitation occured 9000 during gel preparation even in systems with very high amounts of titanium. It a, is worthy of mention that our products are quite different from those previous ~ 6000 ~ _ F reported by E1 Haskouri et al. [9]. In our case, most of the samples exhibit at .9 least three well-resolved reflections in ~ 3000 .;> the 20 range between 2-6 ~ (Figure 1), B which can be indexed to an ordered hexagonal lattice typical of MCM-41 0 6 11 16 [10]. It reveals that following the new 20( ~) synthetic route highly ordered MCM-41 titanosilicates could be hydrothermally Figure 1. XRD patterns of the calcined samples synthesized within a relatively wide A-F in Table 1 (Offsets: vertically by 1000 CPS, composition range. horizontally by 1.0 degree). , ,,,,~
;j
Table 1. Influence of gel composition on crystallization of mesoporous titanosilicate. Sample Gel molar composition Phase Crystallinity ~ (%) n(SiO~) n(TiO?) n(CTABr) n(TBAOH) n(NH3) n(HzO) A 1.00 0.00 0.50 0.02 9.20 130 MCM-41 100 B 0.95 0.05 0.50 0.03 9.20 130 MCM-41 99 C 0.90 0.10 0.50 0.03 9.20 130 MCM-41 90 D 0.85 0.15 0.50 0.05 9.20 130 MCM-41 86 E 0.82 0.18 0.50 0.05 9.20 130 MCM-41 80 F 0.80 0.20 0.50 0.06 9.20 130 MCM-41 68 G 0.85 0.15 0.50 0.05 6.00 130 MCM-41 69 H 0.85 0.15 0.50 0.05 11.00 130 MCM-41 70 I 0.85 0.15 0.05 0.05 9.20 130 Amorphous J 0.85 0.15 0.10 0.05 9.20 130 MCM-41 72 K 0.85 0.15 0.70 0.05 9.20 130 MCM-41 76 L 0.85 0.15 0.50 0.05 5.70 80 MCM-50 M 0..85 0.15 0.50 0.05 7.10 100 MCM-41 85 N 0.85 0.15 0.50 0.05 36.80 520 MCM-41 85 a. Counted on MCM-41 phase compared to sample A after calcination.
170 A careful XRD examination of the as-synthesized and calcined products was also performed at high angle area. However, no distinct peaks were observed in the 20 range between 20-80 ~ which implies the absence of bulky crystalline TiO2 (i.e., anatase and rutile) and titanium silicate. This result suggests that these materials are probably chemically homogeneous. 3.2.
Framework IR Shown in Figure 2 is the framework IR spectrum of as-synthesized sample D. The band at 1080 cm ~ can be ascribed to asymmetric stretching of [SiO4] tetrahedra, while the bands at 459 cm ~ and 800 cm ~ can be assigned to bending of framework Si-O bonds. To our surprise, two weak bands centered at 560 cm ~ and 1237 cm ~ respectively are also observed, which are rarely seen in previous literatures concerning mesoporous materials. The former band characterizes the double-rings' vibrations of external [SiO4] tetrahedra in MFI or MEL structure [ 11 ]. In our study, TBAOH was used as a hydrolysis agent, therefore it is possible that TBA + templated the formation of MFI or MEL structure during crystallization. It suggests that at least part of the [TO4] (T=Ti, Si) tetrahedra within the walls of the assynthesized products is highly cross-linked. This has been demonstrated very recently by two groups separately but using tetraethylammonium or tetrapropylammonium hydroxide as a hydrolysis agent [12,13]. The presence of TBA + resulted in a more ordered and condensed wall structure than those of conventionally prepared ones. However, no absorption related to TiOz or TiO(OH)2 species is detected, which indicates that Ti well disperses in the assynthesized titanosilicate with very high amounts of titanium. An IR band around 960 cm ~ is also observed in Figure 2, which is often assigned to a lattice defect and is correlated with the substitution for silicon with metal ions in the silica framework [1-8]. However, recent work suggests that this band corresponds to a Si-O vibration in a Si-OR (R=H, tetraalkylammonium) group in siliceous materials (e.g., Al-beta and pure MCM-41 silica) [ 14,15]. Nevertheless, there is a controversy on the origin of this IR band, we attentively exclude its appearance as an evidence of the incorporation of Ti into the framework of MCM-41.
1.2
0.8
f ............................................................... ,'-:'. 0.9
.~ 0.6
.:~.4
E r,r
O
DO
< 0.3
~.2 0.0
I
I
I
I
I
I
I
I
0'000 Wavenumber (cm")
Figure 2. Framework IR spectrum of as-synthesized sample D
300 400 2(nm)
500
Figure 3. UV-vis diffuse reflectance spectrum of calcined sample D
171
3.3.
UV-vis DRS UV-vis diffuse reflectance spectroscopy (DRS) is an especially useful technique to characterize the local titanium environment in titanosilicates [ 16]. Figure 3 depicts the UV-vis DRS of calcined sample D. Two absorption bands can be distinguished between 190-400 nm. The band centered at 230 nm corresponds to tetrahedrally coordinated Ti species that substitute for Si in the silica framework, whereas the band around 285 nm probably arises from five- and six-coordinated Ti species [17]. As tetrahedrally coordinated Ti can be hydrated and generates five- and six-coordinated Ti species, it suggests from the UV-vis DRS that more than half amount of titanium may reside in the mesoporous framework, though we can not exclude the existance of partially polymerized Ti species in the walls. However, the absence of a distinct absorption around 330 nm indicates that no anatase-like phases are formed in such a Ti-rich mesoporous titanosilicate upon calcination [16]. 3.4.
Catalytic property The catalytic activity of these solids in the selective oxidation of 4-methylphenol in the presence of dilute hydroperoxide was tested in a glass flask. In a typical reaction, 1.0 g of calcined sample D, 1.0• .2 mol of 4-methylphenol, 1.0• .2 mol of H202 and 100 mL of distilled water were mixed and stirred at 353 K. The results obtained after 5 h of reaction indicated that the catalyst was highly selective. A conversion of 37.6% based on 4methylphenol was reached and 4-methyl catechol was the sole product. Such a preliminary result reveals that sample D is highly catalytically active, which suggests that Ti ions are tetrahedrally incorporated into the MCM-41 framework. In summary, our results unambiguously demonstrate that, by a separate hydrolysis procedure during gel preparation, titanium can be effectively prevented from formation of indissoluble titanium species in the synthesis mixture at very high titanium content, thus highly ordered MCM-41 titanosilicates can be hydrothermally synthesized even from a gel with n(Ti)/n(Si) up to 1/4 and a relatively low template content. During crystallization, titanium ions were partially incorporated into the MCM-41 framework. The addition of TBAOH resulted in a more cross-linked and ordered wall structure. With the advantages of large pore diameter and ordered framework structure, the as-synthesized mesoporous titanosilicates may find special usage in catalysis field.
4.
ACKNOWLEDGMENTS
The financial support of this research by both the National Natural Science Foundation of China (through Grants No. 29733070 and No. 50102001) and the Natural Science Foundation of Tianjin, China (through Grant No. 13608111) is gratefully acknowledged.
REFERENCES 1. G. Perego, G. Bellussi, C. Corno, M. Taramasso, F. Buonomo and A. Esposito, Stud. Surf. Sci. Catal., 28 (1986) 129. 2. M. S. Rigutto and H. van Bekkum, Appl. Catal. A, 68 (1991) L 1. 3. D.P. Serrano, H. X. Li and M. E. Davis, J. Chem. Soc., Chem. Commun., (1992) 745.
172 4. M.W. Anderson, O. Terasaki, T. Ohsuna, A. Philippou, S. P. Mackay, A. Ferreira, J. Rocha and S. Lidin, Nature, 367 (1994) 347. 5. X.-H. Tang, R.-Z. Zhu, L.-R. Pan and H.-X. Li, Chem. J. Chinese Universities, 21 (2000) 517. 6. A. Corma, M. T. Navarro and J. Perez-Pariente, J. Chem. Soc., Chem. Commun., (1994) 147. 7. P.T. Tanev, M. Chlbwe and T. J. Pinnavaia, Nature, 368 (1994) 321. 8. K.A. Koyano and T. Tatsumi, Chem. Commun., (1996) 145. 9. J. E1 Haskouri, S. Cabrera, M. Gutierrez, A. Beltr~n-Porter, D. Beltr~.n-Porter, M. D. Marcos and P. Amor6s, Chem. Commun., (2001) 309. 10. C.T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710. 11. E.M. Flanigen, H. Khatami and H. A. Szymanski, Adv. Chem. Ser., ACS, 101 (1971) 201. 12. Y. Liu, W. Zhang and T. J. Pinnavaia, Angew. Chem. Int. Ed., 40 (2001) 1255. 13. Z. Zhang, Y. Han, L. Zhu, R. Wang, Y. Yu, S. Qiu, D. Zhao and F. Xiao, Angew. Chem. Int. Ed., 40 (2001) 1258. 14. C.B. Dartt, C. B. Khouw, H.-X. Li and M. E. Davis, Microporous Mater., 2 (1994) 425. 15. T. Blasco, A. Corma, M. T. Navarro and J. Perez-Pariente, J. Catal., 156 (1995) 65. 16. A. Tuel, Microporous Mesoporous Mater., 27 (1999) 151. 17. F. Geobaldo, S. Bordiga, A. Zecchina, E. Giamello, G. Leonfanti and G. Petrini, Catal. Lett., 16 (1992) 109.
Studies in Surface Science and Catalysis 141 A. Sayari and M. Jaroniec (Editors) 9 2002 Elsevier Science B.V. All rightsreserved.
Synthesis
and
Characterization
173
of
Ti-containing
Mesoporous
Alumina
M o l e c u l a r Sieves Chun Yang a.b*and Xi Li a a College of Chemistry and Environmental Science, Nanjing Normal University, Nanjing, 210097, P.R.China u National Laboratory of Molecular & Biomolecular Electronics, Southeast University, Nanjing, 210096, RR.China
Ti-containing mesoporous alumina molecular sieves with a structure of MSU-2 have been synthesized using metal alkoxides as titanium and aluminum sources and Triton X-100 as templating surfactant, respectively. The structure of the products and the state of Ti species were characterized by XRD, TEM, N2-sorption, UV-vis DRS and Laser Raman Spectroscopy. It is found that the surface area and the pore volume of sample increase when Ti is incorporated, suggesting an effect of Ti on stabilizing the alumina framework. It is also shown that most of Ti exists in the framework as an isolated mononuclear species at Ti/Al_<6%. As Ti content increases, polymerized Ti species and even TiO2 domains form. But these domains grow so difficultly within mesoporous walls that they graft to the surface of alumina walls at a higher Ti content level, leading to some degree of pore blocking. However, up to Ti/AI = 33%, no well-defined bulk TiO2 is tbund, meaning that Ti species can be dispersed better in mesoporous alumina than in conventional TiO2-A1203 composite.
1. INTRODUCTION Because of their large pore size different from traditional molecular sieves, mesoporous molecular sieve materials have attracted considerable attention for their potential use in catalytic transformation of large molecules, material preparation and as hosts lbr supramolecular assembly. Except silica and aluminosilicate, various metal oxides with mesostructure have also been synthesized. Mesoporous alumina molecular sieve is one of them. It has been reported that the mesoporous aluminas can be synthesized by several templating routes [1-5], and the pore sizes of the products are 2-10 nm. Among these routes, a nonionic one, which employs polyethylene oxide (PEO) and aluminum alkoxide as templating surfactant (N ~ and inorganic aluminum precursor (I~ respectively, was adopted by
174 Pirmavaia's group to successfully synthesize the mesoporous aluminas with hexagonal-like symmetry and wormhole channel motifs [4,5]. These materials are named as MSU-X. The advantage of this N~ ~ pathway is that the surfactant is inexpensive and biodegradable. "l'i-containing aluminas (titania-alumina composites) have been widely used as catalysts, catalyst carriers or ceramic materials. Much research work has focused on the study of these materials [6-8]. Special attention has been riveted on the state of Ti species and the dispersity of Ti atoms on alumina surface or in alumina matrix. However, the properties of these materials are limited because they possess only textural porosity and lack the selective framework pore structure characteristic of a molecular sieve. Mesoporous aluminas have regular channels on the scale of nanometer and large specific surface area; therefore, the preparation of mesostructured Ti-containing aluminas by incorporating Ti atoms into the mesoporous aluminas is expected to endow the materials with fi'amework-confined pore structure and higher Ti dispersing degree. These new composites will undoubtedly possess greater space for application in catalysis and material area. In the present work, Ti-containing mesoporous aluminas with mesostructure of MSU-2 were synthesized. Their structures were characterized by XRD, TEM, N2adsorption/desorption. The information from UV-vis Diffuse Reflectance and Laser Raman spectroscopy showed that Ti species were dispersed better in mesoporous alumina than in conventional TiO2-A1203 composite.
2. EXPERIMENTAL
2.1. Synthesis of samples The synthesis of MSU-2 mesoporous alumina was carried out according to the method in Ref [5]. Aluminum tri-sec-butoxide and Triton X-100 were used as aluminum source and templating surfactant, respectively. The molar composition of the reaction mixture was lsurfactant : 5A1 : 20H20. Ti-containing mesoporous aluminas were synthesized following the same method but using titanium isopropoxide as a titanium precursor. A specific procedure was as follows: a calculated amount of aluminum tri-sec-butoxide and titanium isopropoxide were mixed and stirred for 6 h. Upon completion of mixing, adding Triton X-100 into the mixture and introducing deionized water slowly under stirring to make the molar composition of reaction mixture be 1Triton X-100 9 5A1 9 xTi " 20H20, where x is 0.1, 0.3, 0.95 and 1.65, corresponding to Ti/Al = 2%, 6%, 19% and 33% (molar ratio). The resulting gel was diluted with sec-buyl alcohol and allowed to react at room temperature for 19 h. After the reaction, the solid product was filtered and washed with absolute ethanol, and followed by drying sequentially at room temperature for 16 h and at 100~ for 6 h. With increasing Ti content, the sample was designated in turn as [Ti]-Al203-1, 2, 3 and 4. The surfactant in all samples was removed by calcining the samples in air at 500~ for 6 h after increasing the temperature to 500~ at 1~ of heating rate.
175 2.2. Characterization XRD (X-ray powder diffraction) patterns were taken on a D/max-rC diffractometer using Cu Kcz radiation. Low temperature nitrogen sorption measurements were carried out on Micromeritics ASAP 2000 porosimeter. The surface areas were determined by the BET method. The pore volumes and the pore size distributions were obtained from single-point and the BJH methods, respectively. Before the measurement, the calcined sample was degassed at 300~ for 4-5 h until the vacuum of system was above 5x 10.3 mmHg. TEM (Transmission election microscopy) were performed with a JEOL JEM-2000EX microscope working at 120 kV. The samples fbr TEM were prepared by suspending the powder in absolute ethanol and by depositing a few drops of the suspension on a Cu grid covered with a thin carbon film. UV-vis DRS (UV-vis diffuse reflectance spectra) were obtained on a Shimadzu UV-240 spectrophotometer. BaSO4 reference was used for the measurements. Laser Raman Spectra were measured on a Bruker RFS-100 spectrometer equipped with a Nd:YAG laser operating at a wavelength of 1064 nm. Tile number of scans was 100 and the resolution of the spectrometer was 4 cm -~
3. RESULTS AND DISCUSSION 3.1. XRD and T E M
Typical XRD patterns of MSU-2 alumina and Ti-containing sample are shown in Fig.1. Only a broad single peak ((100) peak), characteristic of disordered, hexagonal-like packing oi" channels [4], is observed in the range of 20 = 0.50-8~ The intensity of the peak greatly increases after removing the template (Fig la and b). However, the location of the peak can not be determined accurately because the d spacing is so large that the XRD line overlap with tile scattering at low angle and no whole (100) peak is observed. This is in agreement with Pinnavaia's observation that d~00of the alumina sample prepared with the same surfactant is greater than 9 [5]. XRD pattern of Ti-containing sample is similar to that of pure alumina (Fig l c). Introduction of Ti, however, decreases the intensity of XRD line. When Ti content is increased to Ti/AI = 33%, the intensity of" (100) peak is much lower than that of pure alumina (not shown here). This seems to suggest that a part of Ti have become extra-framework species at this content level, thereby resulting in the decrease in purity of mesophase and the lowering in diffraction intensity of (100) peak. But no TiO2 phase is detected by wide-angle XRD in the sample. The feature of channel structure shown by XRD is confirmed by TEM images in Fig 2. It can be seen that the particle of sample contains a large number of channels and the packing of channel system appears to be random and disordered though more or less regular in diameter. Since PEO-bascd surfactants adopt spherical to long "wormlike" micellar structures in
176
Fig.1 XRD patterns of samples a) as-synthesized AlzO3, b) calcined AI203, c) calcined [Ti]- A1203-2
Fig.2
TEM images of calcined samples (amplified by 300 thousand times) a) AI203, b) [Ti]- 11203-2
aqueous solution [9,10], the disordered channel system of MSU-2 samples should be mainly attributed to the formation of wormlike micelles in addition to a weak interaction between the organic templates and the inorganic species in N~ ~ assembly pathway. This character of channel packing still remains after Ti atoms are introduced.
177 3.2. N2-adsorption/desorption Fig.3 provides N2-adsorption/desorption isotherms of calcined samples. For pure alumina (Fig.3a), a broad step resulting from the condensation of adsorbate within framework mesopores occurs above P/Po = 0.5 and is accompanied by a large hysteresis loop. These features denote that the sample possesses a large pore size and broad distribution of diameter. The isotherm of Ti-containing sample with less Ti content is similar to that of pure alumina (Fig.3b). However, when Ti content is increased to Ti/AI = 33% (Fig.3c), the pore filling step in the adsorption curve becomes more narrow and shifts to a lower P/P0 value. The hysteresis loop becomes also smaller. These reveal a decrease in pore size and a narrowing in distribution of diameter, and can be more clearly seen from Fig.4. The data for pore diameter in Table 1 further show that pore size increases when less Ti are incorporated; but it decreases as Ti content increases, similar to the case of Ti-containing mesoporous silica [ 11 - 13]. Moreover, it can be found l'rorn Table 1 that the surface area and the pore volunle increase after Ti are incorporated. This phenomenon has also been observed tbr some TiO,-
o ~ B
3111121111-
I.
IO0O
.
. r~ / !
1.2
.
.
.
i
_
i
0
0.8
c
-d 0.4
/'i
/ 0
0.0
..
.,'/',
!/,,
.~
0.2
.,
,, . . . . .
0.4
0.6
0~.8
PIPe
Fig.3 N2-adsorption/desorption isotherms of calcined samples, a) A1203, b) [Ti]-A1203 -2, c) [Ti]- A1203-4
o.o
~-=-~
! t\ ':
",
. . . .s. . .
.r\
,,\
I i
',\ ~o
diatneter
,' : 40
'
'~o ....
,' ,;o
"
,
'
/ nm
Fig.4 Pore size distribution of calcined samples. A1203, - - [Ti]-A1203_2 ' [Ti]- A1203-4
178 Table 1 Somc paranactcrs of [Ti]-Ai20~ mcsoporous molecular sieves SaEv Pore volume Pore size sample Ti/Ai Ti wt% (m2. .gl) (mL. g~) (nm) .
.
.
AI203 [Ti]-AI203-1 [Ti]-AI203-2 [Ti]-AI203-3 [Ti]-AlzO3-4
.
.
.
.
2% 6% 19% 33%
.
.
.
1.8% 5.2% 13.8% 20.4%
.
232 325 367 359 376
0.42 0.59 0.55 0.57 0.48
4.1 4.5 4.1 3.8 3.4
AI203 composites and mesoporous silicas [8,11-13]. It has been reported that MSU-X aluminas are not thermal stable [14]. The structural collapse occurs during the calcination, leading to the loss of surface area and porosity. One improving approach is to dope MSU-X aluminas with rare earth metal ions, such as Ce 3' or La 3+, which dramatically enhance the surface area and the pore volume of the calcined samples. The stabilization mechanism was proposed to be the replacement of A13+by rare earth cations, which reduces the lability of the framework wall of MSU-X aluminas. For our samples here, a similar increase in surface area and porosity occurs after introducing Ti, meaning that Ti4+ cations are also effective in stabilizing the l'ramcwork wall of MSU-X almninas against collapse at elevated temperature. On the other hand, this fact also signifies an entrance of partial Ti 4+ cations into the framework by substituting A134. In the pore size distribution determined from the desorption isotherm (Fig.4), pure alumina sample displays textural pores with the diameter greater than 100 nm (Fig.4,---.line); but these pores disappear after Ti are introduced (Fig.4, . line). This fact also evidences that there exist a small amount of amorphous particles caused by collapse in pure alumina, resulting in large interparticle pores. These particles decrease or disappear upon the incorporation of Ti. However, for the sample with Ti/A1 --- 33%, both the pore diameter and the pore volume noticeably decrease (see Table 1), indicating some degree of pore blocking. This may be due to a removal of a part of Ti species from the framework to form TiO2 clusters depositing on the surface of pore wall at such a high Ti content level. Some small particles of TiO2 clusters departing from the surface may create interparticle pores and result in a small peak at 50-70 nm in pore distribution curve of [Ti]-AI203-4 sample ( Fig.4, ---line). 3.3. UV-vis D RS UV-vis DRS of pure alumina and Ti-containing alumina are shown in Fig.5. Pure assynthesized alumina exhibits two absorption bands at ca. 230 nm and ca. 280 nm, respectively; but they disappear after the calcination (Fig.5a and b), suggesting these two bands caused by Triton X-100 templating surfactant because of the presence of large rt bond, such as aromatic ring, in its molecules. Similarly, for as-synthesized Ti-containing sample (Fig.5c), two shoulder bands on both sides of the main absorption band also result from the template, while the main band around 240 nm indicates the incorporation of photoactive Ti species into the sample. Upon the calcination, the shoulder bands disappear and the main band widens due to
179
a -.._...
200
!
|
300
400
,
,
500
k/nm Fig.5 UV-vis DRS of samples a) as-synthesized A1203, b) calcined A1203, c) as-synthesized [Ti]-A1203-2, d) calcined [Ti]-A1203-2
200
!
I
300
400
500
)~/nm Fig.6 UV-vis DRS of calcined samples a) [Ti]-AI203-1, b) [Ti]-AI203-2, c) [Ti]-A1203-3, d) [Ti]-A1203-4
the increase of relative Ti content (Fig.5d). UV-vis spectroscopic investigations of Ti-containing mesoporous silicas and 'l'iO2-SiO 2 composites [11,13,15-18] have assigned the UV band at ca. 330 nm to bulk TiO2 (anatase), and the band centred at 220 nm to isolated Ti atoms in tetrahedral sites. The latter shills towards greater wavelength with increasing Ti content, which is attributed to the formation of polymerized Ti species (Ti-O-Ti species) or isolated Ti species with higher coordination numbers. Pacheco-Malagon and co-workers studied TiO2--AI203 composites prepared by hydrolysis of metal alkoxides [ 19]. Their results showed that for the sample with Ti/A1 >_ 7.5%, Ti species in the composites aggregated into oxide domains with radius >__0.8 nm and an evident absorption band appeared at 300-320 nm in UV-vis spectra. When Ti content was
180 increased to Ti/A1 > 17.5%, the further growth of titania domains in Al203 matrix was difficult. Thus, a fraction of Ti dispersed on A1203 support or departed from the support as individualized TiO2 crystalline particle s, leading to a significant pore blocking. The UV-vis spectra of our calcined samples with different Ti content are shown in Fig.6. For the samples with Ti/A1 < 6% (Fig.6a and b), an UV absorption band centred at ca.225 mn is presented, indicating most of Ti atoms existing in the framework as an isolated mononuclear TiOx species. For Ti/A1 - 19 (Fig.6c), the UV band shifts towards greater wavelength, suggesting the formation of polymerized Ti species and even TiO2 domains with increasing Ti content. When Ti/A1 ratio is as high as 33% (Fig.6d), the TiOz domains further grow so that a part of absorption edge shifts over 300 nm. Combining the data of pore volume and pore diameter, we may conclude that at such a high Ti content level, a fraction of TiO2 clusters remove from the alumina framework to become extra-wall dispersed TiO2. However, as shown in Fig.6, up to Ti/A1 = 33%, no well-defined absorption band is observed above 300 nm, suggesting that the size of TiO2 domain in our Ti-containing samples is smaller than that in TiO2-AI20~ composites reported by Pacheco-Malagon et al. That is to say, the dispersity of 'l'i species in mesoporous aluminas is higher than that in composite oxides. On the other hand, it is also seen from above results that the growth of TiO2 domains in the mesoporous alumina framework is difficult and consequently limited although their sizes are smaller. This probably arises from the thinner wall of mesoporous alumina as compared with the alumina matrix in composite oxides.
d
b
1000
800
600 cm
*
400
200
-1
Fig.7 Raman spectra of calcined samples a) [Ti]-A1203-4, b) [Ti]-a1203-3, c) [Ti]-a1203-2, d) [Ti]-al203-1,
181 3.4. Laser Raman spectroscopy
The Raman spectrum of anatase shows absorptions at 639, 516, 400 and 144 cm 1 [18. 20]. Among these absorptions, the band at 144 cm 1 has the greatest intensity. In Ti-containing zeolites, the presence of multinuclear TixOyclusters also provokes this band in spectrum. Therefore, it is considered as a sensitive indicator of polymerized TiO 2 clusters [20]. The study about TiO2-A1203 composite oxides by Luo et al. [8] showed that, when TiO2 content reached 10%, i.e., Ti/A1 ratio was ca.7%, a distinct 144 cm-' band (shifting to 156 cm") appeared in the Raman spectrum of the sample. This indicates the formation of TiO2 clusters in the form of anatase. Raman spectra of our Ti-containing samples are depicted in Fig.7. When Ti/A1 ratio is 19 or higher, small TiO2 clusters form in the samples, as confirmed by a very weak absorption at 144 cm -~ (designated by asterisk), in accordance with above results from UV-vis DRSI In addition, the Ti content in our sample is much higher than that in TiO2-A1203 composite reported by Luo et al. when the 144 cm ~ band appears; while the intensity of the band is lower tbr our samples than that for the composites. This suggests once again that Ti species in mesoporous alumina have a higher dispersity.
REFERENCES
1. Q-S. Huo, D. I. Margolese, U. Ciesla, P-Y Feng, T. E. Gler, R Sleger, R. Leon, R M. Petroff, F. Schuth, G. D. Stucky, Nature. 368 (1994) 317 2. F. Vaudry, S.Khodabandeh, M. E. Davis, Chem. Mater., 8 (1996) 1451 3. M.Yada, M. Machida, T. Kijima, Chem. Commun., (1996) 769 4. S.A. Bagshaw, E. Prouzet, T. J. Pinnavaia, Science, 269 (1995) 1242 5. S.A. Bagshaw, T. J. Pinnavaia, Angew. Chem. Int. Ed. Engl., 35 (1996) 1102 6. Z-B. Wei, Q. Xin, X-X Gao, E.L. Sham. R Grange, B. Delmon, Appl. Catal., 63 (1990) 305 7. M.Anpo, T. Kawamura, S. Kodama, K. Maruya, T. Onishi, J. Phys. Chem., 92 (1988) 438 8. S. Luo, L. Gui, Mat. Res. Sco. Symp. Proc., 371 (1995) 303 9. B. Chu, Langmuir, 11 (1995) 414 10. Z. Lin, L. E. Scriven, H. T. Davis, Langmuir, 8 (1992) 2200 11. O. Franke, J. Rathousky, G. Schulz-Ekloff, J. Starek, A. Zukal, Stud. Sure Sci. Catal., 84 (1994) 77 12. 13. 14.
15. 16.
A. Corma, M. T. Navarro, J. Perez-Pariente, F. Sanchez, Stud. Sure Sci. Catal.. 84(1994) 69 S. Gontier, A. Tuel, Zeolites, 15 (1995) 601 W-Z. Zhang, T. J. Pinnavaia, Chem. Commun., (1998) 1185 W-Z. Zhang, M. Froba, J-L. Wang, P. T. Tanev, J.