CHEMICAL ENGINEERING METHODS AND TECHNOLOGY
LANGMUIR MONOLAYERS IN THIN FILM TECHNOLOGY
No part of this digital document may be reproduced, stored in a retrieval system or transmitted in any form or by any means. The publisher has taken reasonable care in the preparation of this digital document, but makes no expressed or implied warranty of any kind and assumes no responsibility for any errors or omissions. No liability is assumed for incidental or consequential damages in connection with or arising out of information contained herein. This digital document is sold with the clear understanding that the publisher is not engaged in rendering legal, medical or any other professional services.
CHEMICAL ENGINEERING METHODS AND TECHNOLOGY Additional books in this series can be found on Nova‟s website under the Series tab.
Additional E-books in this series can be found on Nova‟s website under the E-book tab.
NANOTECHNOLOGY SCIENCE AND TECHNOLOGY Additional books in this series can be found on Nova‟s website under the Series tab.
Additional E-books in this series can be found on Nova‟s website under the E-book tab.
CHEMICAL ENGINEERING METHODS AND TECHNOLOGY
LANGMUIR MONOLAYERS IN THIN FILM TECHNOLOGY
JENNIFER A. SHERWIN EDITOR
Nova Science Publishers, Inc. New York
Copyright © 2011 by Nova Science Publishers, Inc. All rights reserved. No part of this book may be reproduced, stored in a retrieval system or transmitted in any form or by any means: electronic, electrostatic, magnetic, tape, mechanical photocopying, recording or otherwise without the written permission of the Publisher. For permission to use material from this book please contact us: Telephone 631-231-7269; Fax 631-231-8175 Web Site: http://www.novapublishers.com
NOTICE TO THE READER The Publisher has taken reasonable care in the preparation of this book, but makes no expressed or implied warranty of any kind and assumes no responsibility for any errors or omissions. No liability is assumed for incidental or consequential damages in connection with or arising out of information contained in this book. The Publisher shall not be liable for any special, consequential, or exemplary damages resulting, in whole or in part, from the readers‟ use of, or reliance upon, this material. Any parts of this book based on government reports are so indicated and copyright is claimed for those parts to the extent applicable to compilations of such works. Independent verification should be sought for any data, advice or recommendations contained in this book. In addition, no responsibility is assumed by the publisher for any injury and/or damage to persons or property arising from any methods, products, instructions, ideas or otherwise contained in this publication. This publication is designed to provide accurate and authoritative information with regard to the subject matter covered herein. It is sold with the clear understanding that the Publisher is not engaged in rendering legal or any other professional services. If legal or any other expert assistance is required, the services of a competent person should be sought. FROM A DECLARATION OF PARTICIPANTS JOINTLY ADOPTED BY A COMMITTEE OF THE AMERICAN BAR ASSOCIATION AND A COMMITTEE OF PUBLISHERS. Additional color graphics may be available in the e-book version of this book.
LIBRARY OF CONGRESS CATALOGING-IN-PUBLICATION DATA Langmuir monolayers in thin film technology / editors, Jennifer A. Sherwin. p. cm. Includes bibliographical references and index. ISBN 978-1-61209-188-4 (eBook) 1. Thin films, Multilayered. I. Sherwin, Jennifer A. QC176.9.M84L365 2010 621.3815'2--dc22 2010041312
Published by Nova Science Publishers, Inc. † New York
CONTENTS Preface
vii
Chapter 1
Carbons and Clays for Heavy Metals Removal – A Review of Latest Literature John U. Kennedy Oubagaranadin and Z.V.P. Murthy
Chapter 2
Molecular Organization of Thermotropic Liquid Crystals and Their Mixtures with Azo Dyes in Langmuir and Langmuir-Blodgett Films Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
Chapter 3
Atomic Force Microscopy Characterization of Lipid/ Protein Nanostructures Formed in Langmuir-Blodgett Films Yih Horng Tan and Keith J. Stine
Chapter 4
Langmuir Monolayers in Biosensors Jadwiga Sołoducho and Joanna Cabaj
Chapter 5
Adsorptive Characteristics of Bovine Serum Albumin onto Cationic Langmuir Monolayers of Sulfonated Poly (Glycidylmethacrylate)Grafted Cellulose: Mass Transfer Analysis, Isotherm Modeling and Thermodynamics T. S. Anirudhan and P. Senan
Chapter 6
Index
Electrochemistry of Polymeric Thin Films Prepared by Langmuir-Blodgett Technique Paolo Bertoncello
1
51
101 131
151
177 201
PREFACE The Langmuir-Blodgett (LB)technique for the preparation of ultrathin films of various organic, metallorganic, and polymeric compounds play an increasingly important role as a means or organizing molecular materials at the microscopic level. The LB technique has many potential applications in molecular electronics, nonlinear optics and conducting thin films. This book presents current research from across the globe in the study of Langmuir Monolayers, including the study of thermotropic liquid crystals and binary mixtures of dichroic azo dye/liquid crystal in Langmuir and Langmuir-Blodgett films; proteo-lipidic nanostructures generated via the Langmuir-Blodgett film method; Langmuir Monolayers in biosensors; as well as adsorptive characteristics of bovine serum albumin onto cationic Langmuir Monolayers of sulfonated poly-grafted cellulose. Chapter 1 - In this article, various adsorption isotherm models, kinetic models, adsorption thermodynamics and the technical viability of carbons made from different biomaterials and different types of naturally occurring clays for heavy metals removal by adsorption from contaminated water has been reviewed. Natural clays and carbons prepared from waste plant products can be employed for heavy metals removal from aqueous solutions and disposed of with little cost. Modification of these materials can also improve their adsorption capacity. In this review, an extensive literature survey from the past decade on the heavy metals removal characteristics of clays and carbons has been compiled to provide a summary. It is evident from this literature survey that carbons made from biomaterials and clays have demonstrated outstanding removal capabilities for certain metal ions. Some of the highest adsorption capacities reported are: for Cd(II), 180 mg/g by bean husk (Phaseolus vulgaris) carbon; for Cr(VI), 120.48 mg/g by date palm seed wastes carbon; for Pb(II), 279.92 mg/g by carbon made from Euphorbia rigida; for Hg(II), 151.5 mg/g by ZnCl2 activated walnut shells carbon; for Cr(III), 117.5 mg/g by Smectite clay with a small proportion of kaolinite; for Cd(II), 74.07 mg/g by petra clay; for Cu(II), 105.38 mg/g by modified Unye clay; for Pb(II), 104.28 mg/g by natural palygorskite clay; for Cu(II), 909 mg/g by Saudi bentonite. It is important to note that the adsorption capacities of the adsorbents presented in this paper vary, depending on the experimental conditions, characteristics of the individual adsorbent, the extent of chemical modifications, and the concentration of adsorbate. Chapter 2 - In this review articles the results of the study of thermotropic liquid crystals and of binary mixtures of dichroic azo dye/liquid crystal in Langmuir and Langmuir-Blodgett films are presented. The liquid crystals of rod-like shape from various homologous series and nine azo dyes with different molecular structure as well as different values and directions of
viii
Jennifer A. Sherwin
the dipole moment were chosen. It was found that the liquid crystals with the terminal isothiocyanato (–NCS) group are not able to form a compressible monolayer at the water surface. Very short and very long alkyl or alkoxy chains attached to the rigid molecular core also hinder the creation of the stable film. Azo dyes cannot form the Langmuir film themselves; therefore, the liquid crystals 4-n-octyl-4'-cyanobiphenyl (8CB) and trans-4-noctyl(4‟-cyanophenyl)-hexane (8PCH) were used as supporting matrices. The Langmuir films were characterized by the surface pressure-area and surface potential-area isotherms and by Brewster angle microscopy (BAM). The analysis of the isotherms and BAM images of liquid crystals indicated that the organization of the mesogenic molecules at the air-water interface is dependent on their structure and to some extent reflects their ability to form an appropriate mesophase in the bulk. For the binary azo dye/8CB mixtures the miscibility of two components as well as the organization and the packing of molecules at the water surface were determined. The absorption spectra by using natural and linearly polarized light were recorded for both Langmuir and Langmuir-Blodgett films. Information about spectral properties of ultra-thin layers and ability of dye and liquid crystal molecules to form selfaggregates was obtained. The polarized absorption spectra allowed one to determine the alignment of molecules on the quartz surface. Chapter 3 - Recently, much of the emphasis in biotechnology has been on producing nanosystems and nanodevices for a vast range of medical applications, including nanoelectronic biosensors, drug delivery systems, and diagnostic and imaging techniques, to name a few. This chapter reviews the potentially useful creation of proteo-lipidic nanostructures generated via the Langmuir-Blodgett (LB) film method, and their direct characterization by atomic force microscopy (AFM). Following the introductory sections, a brief overview on LB film fabrication on surfaces suitable for AFM will be presented, LB films containing proteins, lipids, and biocompatible amphiphilic molecules will be described, and how they have been studied using various AFM imaging modes. We aim to highlight recent developments that illustrate the unique capability of AFM in elucidating nanometer scale organization and the physicochemical properties of artificially engineered biological membranes through the Langmuir-Blodgett method; as it could potentially open a new pathway toward the development of self-organized nanostructures of technological significance. Chapter 4 - In recent years, the Langmuir-Blodgett (LB) technique for the preparation of ultrathin films of various organic, metallorganic, and polymeric compounds plays an increasingly important role as a means of organizing molecular materials at the microscopic level. The LB technique has many potential applications in molecular electronics, nonlinear optics and conducting thin films. The most important advantage of this method is that the characteristic of the film can be varied by changing various LB parameters, namely, surface pressure of lifting, temperature, barrier speed, dipping speed, molar composition, etc. So it is important to study different molecules having various chromophores with interesting photophysical and electrical properties, confined in the restricted geometry of the LB films to fabricate various molecular electronic devices and also to realize the basic physicochemical processes involved at the mono and multilayer films [1]. Chapter 5 - Investigation on adsorption behaviour of Bovine Serum Albumin (BSA) on polymeric adsorbent materials is critical for many analytical and biomedical applications. In the present study a novel adsorbent poly(glycidylmethacrylate)-grafted-cellulose having sulfonate functional groups (PGMA-g-Cell-SO3H) was prepared by graft copolymerization of
Preface
ix
glycidylmethacrylate (GMA) onto cellulose in the presence of ethyleneglycoldimethacrylate as crosslinker using α,ά-azobisisobutryronitrile as initiator followed by the introduction of sulfonic acid groups through ring opening reaction of the epoxide groups of the grafted GMA with sodium sulfite–isopropanol–water mixture. The original and the modified materials were characterized by means of FTIR, SEM, XRD and BET analysis. Adsorption characteristics of BSA onto PGMA-g-Cell-SO3H were investigated under different optimized conditions of pH, contact time, initial BSA concentration, adsorbent dose and temperature. The maximum value of BSA adsorption was found to be 49.95 and 72.07 mg/g for an initial concentration of 100 and 150 mg/L, respectively at pH 4.5. Kinetic studies showed that the equilibrium conditions were achieved within 3 h. The kinetic data obtained at different concentrations and temperatures were analyzed using a pseudo-first-order and pseudo-second-order equation. The adsorption process followed pseudo-second-order kinetics. The experimental kinetic data were correlated by the external mass transfer and intraparticle mass transfer diffusion models. The intraparticle mass transfer diffusion model gave a better fit to the experimental data. Experimentally obtained isotherms were evaluated with reference to Langmuir, Freundlich and Sips equations. The isotherm data were best modelled by the Langmuir isotherm equation and the maximum monolayer adsorption capacity was found to be 124.85 mg/g at 30 °C. Thermodynamic study revealed an endothermic adsorption process. The negative ΔG° values indicate feasible and spontaneous adsorption of BSA onto PGMA-g-Cell-SO3H. The positive and small value of enthalpy change ΔHo (9.50 kJ/mol) indicates the endothermic nature of adsorption primarily through weak physical forces between adsorbent and adsorbate. The positive and small value of entropy change, ΔSo (185.52 J/mol/K) indicates that the order less nature of adsorption system increases with adsorption of BSA onto adsorbent surface. Also at all temperatures ΔHo
In: Langmuir Monolayers … Editors: Jennifer A. Sherwin
ISBN: 978-1-61122-461-0 ©2011 Nova Science Publishers, Inc.
Chapter 1
CARBONS AND CLAYS FOR HEAVY METALS REMOVAL – A REVIEW OF LATEST LITERATURE John U. Kennedy Oubagaranadin 1,2 and Z.V.P. Murthy*2 1
Department of Ceramic and Cement Technology, PDA College of Engineering, Gulbarga, Karnataka, India 2 Department of Chemical Engineering, S.V. National Institute of Technology, Surat, Gujarat, India
ABSTRACT In this article, various adsorption isotherm models, kinetic models, adsorption thermodynamics and the technical viability of carbons made from different biomaterials and different types of naturally occurring clays for heavy metals removal by adsorption from contaminated water has been reviewed. Natural clays and carbons prepared from waste plant products can be employed for heavy metals removal from aqueous solutions and disposed of with little cost. Modification of these materials can also improve their adsorption capacity. In this review, an extensive literature survey from the past decade on the heavy metals removal characteristics of clays and carbons has been compiled to provide a summary. It is evident from this literature survey that carbons made from biomaterials and clays have demonstrated outstanding removal capabilities for certain metal ions. Some of the highest adsorption capacities reported are: for Cd(II), 180 mg/g by bean husk (Phaseolus vulgaris) carbon; for Cr(VI), 120.48 mg/g by date palm seed wastes carbon; for Pb(II), 279.92 mg/g by carbon made from Euphorbia rigida; for Hg(II), 151.5 mg/g by ZnCl2 activated walnut shells carbon; for Cr(III), 117.5 mg/g by Smectite clay with a small proportion of kaolinite; for Cd(II), 74.07 mg/g by petra clay; for Cu(II), 105.38 mg/g by modified Unye clay; for Pb(II), 104.28 mg/g by natural palygorskite clay; for Cu(II), 909 mg/g by Saudi bentonite. It is important to note that the adsorption capacities of the adsorbents presented in this paper vary, depending on the experimental conditions, characteristics of the individual adsorbent, the extent of chemical modifications, and the concentration of adsorbate.
2
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
1. INTRODUCTION Heavy metals in the environment are not biodegradable and tend to accumulate in living organisms, causing various diseases and disorders. Eleven metals, viz., Pb, Cr, Hg, U, Se, Zn, As, Cd, Co, Cu and Ni, out of 20 classified metals as toxic, are emitted into environment in quantities that pose risks to human health (Kortenkamp et al., 1996). It is known that adsorption is cost effective and efficient in heavy metals removal from solutions. Application of carbons made from plant species and naturally occurring inorganic materials (clays) in heavy metals removal from various industrial effluents or water resources have been reported. Adsorption with clays has become an alternative to traditional methods of industrial wastewater treatment and it is relatively inexpensive, non-hazardous, and may permit recovery of the metals from the adsorbing mass. Adsorbent carbons and clays are different in nature. A pure carbon surface is considered to be non-polar, but in actuality some carbon-oxygen complexes CxO, COx and CxO2 are usually present. When a metal ion is present in solution, surface complexes may be formed by ion exchange between H+ functional groups and metal ions in solution. Such mechanism is consistent with those proposed in earlier investigations (Namasivayam and Periasamy, 1993; Namasivayam and Kadirvelu, 1999). As metal ions are adsorbed onto the carbon, more hydrogen ions are released from the carbon into solution. The hydrogen ion sources are most likely the carboxylic, phenolic, sulfonic and lactonic groups in the carbon. These groups are generally considered to be responsible for cation exchange capacity of carbons (Kadirvelu et al., 2000).
Clays are basically aluminosilicate minerals containing sodium, potassium and calcium, in which magnesium and iron may be substituted for aluminium. The ion-exchange capacity of clays depends on the frame work of Si/Al ratio and decreases as the Si/Al ratio increases. The clays carry a net negative charge due to the broken bonds around the edges of the silicaalumina units that would give rise to unsatisfied charges, which would be balanced by the adsorbed cations. Substitutions within the lattice structure of trivalent aluminum for quadrivalent silicon in the tetrahedral sheet and of ions of lower valence, particularly magnesium for trivalent aluminum in the octahedral sheet, result in unbalanced charges in the structural units of clay minerals (Pehlivan et al., 2006). The process of adsorption is well explained by the well-known two-parameter Freundlich and Langmuir isotherms. However there are a number of other two-parameter, threeparameter and four-parameter models that can explain the adsorption equilibrium data better. Similarly kinetics of adsorption can be represented by a number of rate models. This article provides a collection of these models for the testing of adsorption equilibrium and kinetics data, and an overview of carbons made from bio-materials and clays for heavy metal removal from aqueous solutions based on recent publications (past decade).
2. ADSORPTION ISOTHERMS, KINETICS AND THERMODYNAMICS 2.1. Adsorption Isotherms Adsorption is a surface process that leads to transfer of molecules from a fluid bulk to solid surface. This can occur because of physical forces or by chemical bonds. In most of the
Carbons and Clays for Heavy Metals Removal …
3
cases, this process is described at the equilibrium by means of some equations that quantify the amount of substance attached on the surface given the concentration in the fluid. These equations are called isotherms because of the dependence of their parameters on the temperature, which is one of the most important factors affecting the adsorption. The uptake capacity of an adsorbent at equilibrium is given by:
qe
(C0 Ce ) m /V
(2.1)
where, C0 and Ce are the initial and equilibrium concentration of the adsorbate (mg/L), m is mass of the adsorbent (g) and V is the volume of the solution (L). A brief description of various adsorption isotherm models used by researchers is given below.
2.1.1. Henry Isotherm Henry‟s law is basically a one parameter model and has been applied in many cases (Ho, 2004a). It has the form of equation of a straight line with no intercept. This model normally does not represent the adsorption equilibrium data due to the unavailability of adsorption data in the lower range of metal concentration. In liquid-phase adsorption, the equilibrium adsorption data are normally obtained at higher equilibrium concentrations, where the adsorbent surface is almost at the edge of saturation. High concentrations may suggest the applicability of a model having a linear relationship between qe and Ce at the latter part of the equilibrium isotherm curve. This requisite may be partially fulfilled using Henry‟s law equation with an intercept. The addition of a constant term in Henry‟s law provides the model to integrate the basic characteristics of the equilibrium isotherm curve at the high concentration range. Henry‟s law is given as:
qe K H Ce b
(2.2)
where, KH and b are model constants. This model can be applied for high effluent concentration.
2.1.2. Freundlich Isotherm The Freundlich isotherm (Freundlich, 1907) habitually gives a better fit particularly for adsorption from liquids and can be expressed as:
qe K F Ce
1
n
(2.3)
In this model, the mechanism and the rate of adsorption are functions of the constants n and KF (L/g). For a good adsorbent, 1
4
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
2.1.3. Langmuir Isotherm The Langmuir (1916, 1917, 1918) model assumes uniform energies of sorption onto the surface and no transmigration of adsorbate in the plane of the surface. The Langmuir equation may be written as:
qe
qm K L Ce 1 K L Ce
(2.4)
In this model, qm (mg/g) is the amount of adsorption corresponding to complete monolayer coverage, i.e., the maximum adsorption capacity and KL (L/mg) is the Langmuir constant. It is also a simple expression with interpretable parameters and applicable for monolayer adsorption. For Langmuir type adsorption process, to determine if the adsorption is favorable or not, a dimensionless separation factor, RL, is defined (Hall et al., 1966) as:
RL
1 1 K L C0
(2.5)
If R L >1, the isotherm is unfavorable
RL =1, the isotherm is linear 0< R L <1, the isotherm is favorable
2.1.4. Dubinin-Radushkevich Isotherm The Dubinin-Radushkevich (D-R) adsorption isotherm (Dubinin and Radushkevich, 1966) is given as:
qe qm exp( D 2 )
(2.6)
here, ε (known as Polanyi potential) is given as (Rosene and Manes, 1977):
RT ln 1
1 Ce
(2.7)
where, R is the gas constant, T is temperature and the constant D (mol2/kJ2) given by the following Eq. (2.8), in terms of the mean free energy E (kJ/mol) of sorption per molecule of adsorbate. When the molecule is transferred to the surface of the solid from infinity in the solution, E is given by:
E
1 2D
(2.8)
Carbons and Clays for Heavy Metals Removal …
5
This isotherm is temperature independent and suitable for porous adsorbents.
2.1.5. Temkin Isotherm The derivation of the Temkin isotherm (Temkin and Pyzhev, 1940) assumes that the fall in the heat of sorption is linear rather than logarithmic, as implied in the Freundlich equation. The Temkin isotherm equation assumes that the heat of sorption of all the molecules in the layer decreases linearly with coverage due to sorbent-sorbate interactions, and that the adsorption is characterized by a uniform distribution of the binding energies, up to some maximum binding energy. The Temkin isotherm has generally been applied in the following form:
qe B ln( K T Ce ) where B
(2.9)
RT H o
(2.10)
Here, B is related to the heat of sorption (J/mol), R the gas constant (8.314 J/mol/K) and T the absolute temperature (K) and KT (L/mg) is the equilibrium binding constant corresponding to the maximum binding energy.
2.1.6. Harkins-Jura Isotherm The Harkins–Jura adsorption isotherm can be expressed as (Başar, 2006):
qe
P1 P2 log Ce
(2.11)
where, P1 and P2 are isotherm constants. This model accounts to multi-layer sorption and can be explained with the existence of a heterogeneous pore distribution.
2.1.7. Halsey and Henderson Isotherms The Halsey isotherm (Halsey, 1948) and Henderson isotherm (Henderson, 1952) models explains multilayer sorption. They are generally applied in the following forms, respectively:
ln P3 ln C e qe exp P4 ln(1 C e ) qe P5
1
(2.12)
P6
where P3, P4, P5 and P6 are isotherm constants.
2.13)
6
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
2.1.8. Brunauer-Emmet-Teller Isotherm The Brunauer-Emmet-Teller (BET) isotherm (Brunauer et al., 1938) is an S-shaped isotherm, given as:
qe
q m kCe (C0 Ce )[1 (k 1)(Ce / C0 )]
(2.14)
The constant k is large as compared to unity and, therefore, the isotherm consists of two regions, i.e. low and high concentration regions. This isotherm is applicable for multilayer adsorption.
2.1.9. Redlich-Peterson Isotherm Redlich-Peterson sorption isotherm (Redlich and Peterson, 1959) is an empirical isotherm incorporating three parameters. It combines elements from both the Langmuir and Freundlich equations, and the mechanism of sorption is a hybrid and does not follow ideal monolayer sorption. This model is given as:
qe
K RP C e 1 a RP C e
(2.15)
Here KRP is Redlich-Peterson isotherm constant (L/g), aRP is also a constant (L/mg)1/ and is an exponent that lies between 0 and 1. For = 1, Eq. (2.15) reduces to Langmuir equation and for = 0, it reduces to Henry‟s equation. This three-parameter model approaches the Freundlich model at high concentrations and is in agreement with the low concentration limit of the Langmuir equation.
2.1.10. Sips Isotherm Recognizing the problem of the continuing increase in the adsorbed amount with an increase in concentration in the Freundlich equation, Sips (1948) proposed an equation similar in form to the Freundlich equation, but it has a finite limit when the concentration is sufficiently high. Sips isotherm has the following form:
qm ( K S Ce ) qe 1 ( K S Ce )
(2.16)
where, qm is the maximum adsorption capacity (mg/g), KS is the Sips isotherm constant (L/g) and is the model exponent. At low sorbate concentrations, Sips equation reduces to the Freundlich isotherm. At high sorbate concentrations, Sips model predicts monolayer sorption capacity and distinctiveness of the Langmuir isotherm.
2.1.11. Radke-Prausnitz Isotherm The Radke-Prausnitz isotherm model (Radke and Prausnitz, 1972) can be expressed as:
Carbons and Clays for Heavy Metals Removal …
qe
q m K rp Ce
7
(2.17)
(1 K rp Ce )
where, Krp is Radke-Prausnitz model constant and the model exponent. It represents the Langmuir model for α = 1 and Henry‟s model for α = 0.
2.1.12. Tóth Isotherm Tóth (2000) has modified the Langmuir equation to reduce the error between experimental data and predicted values of equilibrium adsorption data. The application of this equation is best suited to multi-layer adsorption similar to BET isotherm which is a special type of Langmuir isotherm and has very restrictive validity. The Tóth model can be represented as:
qe
q m K Th Ce
[1 ( K Th Ce ) ]
1
(2.18)
where KTh is the Tóth model constant and δ is the model exponent. For δ = 1, this isotherm reduces to the Langmuir adsorption isotherm.
2.1.13. Fritz–Schluender Isotherm (3-Parameter) The Fritz–Schluender equation (Fritz and Schluender, 1974) has the following form:
qe
q m K FS C e 1 qm Ce
(2.19)
where KFS the Fritz-Schluender equilibrium constant (L/mg), and λ is the Fritz–Schlunder model exponent.
2.1.14. Fritz–Schluender Isotherm (4-Parameter) Fritz–Schluender (Fritz and Schluender, 1974) proposed an empirical relation with four parameters to describe equilibrium data and it is Langmuir-Freundlich type of equation.
qe
JC e
K
1 LCe
M
(2.20)
where J and L are the Fritz–Schluender parameters, and K and M are the Fritz–Schluender equation exponents. At high liquid-phase concentrations of the adsorbate, Eq.(2.20) reduces to the Freundlich equation and for K = M = 1, Eq. (2.20) reduces to the Langmuir equation.
2.1.15. Extended Langmuir Isotherm Originally, the Langmuir model was intended for monolayer adsorption with no interaction between adsorbed molecules. Thus, its ability to correlate experimental data is
8
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
limited. The extended Langmuir model (Yao, 2000) is a modified three-parameter version of the Langmuir model, which can provide better fit to the experimental data (Hall et al., 1966).
qe
q m K EL Ce (1 K EL Ce k EL K EL Ce )
(2.21)
where, KEL (L/mg) and kEL (dimensionless) are model parameters. The constant KEL of the model is a coefficient attributed to the affinity between the adsorbent and adsorbate.
2.1.16. Competitive Langmuir Isotherm The difficulties in describing the adsorption of metal ions from wastewater resulted from the presence of several different ions, causing interference and competition on adsorption sites. Therefore, for a wastewater containing two different metal ions, the competitive Langmuir model for two competing ions, can be used in order to express the relationships between the quantity of the first component adsorbed and the concentration of the second component (Ho and McKay, 2000). The model can be expressed as:
q e ,i
q m , i K i C e ,i 1 K i C e ,i K j C e , j
(2.22)
where, Ki and Kj are model parameters, and the subscripts i and j indicate two different metal ions.
2.2. Adsorption Kinetics Two vital evaluation elements for an adsorption process operation unit are the mechanism and the reaction rate. Solute uptake rate determines the residence time required for completing the adsorption and can be enumerated from kinetic analysis. Numerous attempts were made in formulating a general expression to describe the kinetics of adsorption on solid surfaces for the liquid-solid adsorption system. In 1898, Lagergren presented the pseudo-firstorder rate equation for the adsorption of oxalic acid and malonic acid onto charcoal (Lagergren, 1898; Ho, 2004b). Lagergren‟s kinetics equation may have been the first one in describing the adsorption of liquid-solid systems based on solid capacity. The two kinetic models, namely pseudo-first-order (Lagergren, 1898; Ho, 2004b) and pseudo-second-order (Ho and McKay, 1999) equations have been widely used to describe adsorption data obtained under non-equilibrium conditions. In most of the adsorption kinetic studies, both pseudo-first-order and pseudo-second-order kinetic equations have been commonly employed parallely and one is often claimed to be better than another according to marginal difference in correlation coefficient. As noted by Rudzinski and Plazinski (2006), in the past decades no attempts were made to clearly explain the theoretical origins of these two equations, i.e., current understanding of adsorption kinetics is much less than theoretical description of adsorption equilibrium. A brief description of various kinetic models is given below.
Carbons and Clays for Heavy Metals Removal …
9
2.2.1. Fractional Power Model The fractional power function model (Dalal, 1974) is a modified form of the Freundlich equation and may be expressed as:
qt k F t
(2.23)
where, qt is the amount of metal ion sorbed by sorbent at a time t, while kF and ν are constants with ν < 1. This expression is generally empirical, except for the case in which ν = 0.5, where it becomes indistinguishable from the parabolic diffusion equation.
2.2.2. Pseudo-First-Order Model Pseudo-first-order rate equation is expressed as follows (Lagergren, 1898; Ho, 2004b):
dqt k1 (qe qt ) dt
(2.24)
where, k1 is pseudo-first-order rate constant. After integration and applying boundary conditions t = 0 and qt = 0 to t = t and qt = qe at equilibrium, the Eq. (2.24) becomes
qt qe (1 e k1t )
(2.25)
where, value of k1 can be determined from the slope of the plot of log (qe −qt) versus t.
2.2.3. Pseudo-Second-Order Model Pseudo-second-order rate equation is expressed as (Ho, 2006a,b):
dqt k 2 (q e qt ) 2 dt
(2.26)
where, k2 is pseudo-second-order rate constant. After integration and applying the same boundary conditions t = 0 and qt = 0 to t = t and qt = qe at equilibrium, Eq. (2.26) becomes 2
q k t qt e 2 1 k 2 qe t
(2.27)
In the linear form Eq. (2.27) becomes,
t 1 t = + 2 qt k 2 q e q e
(2.28)
10
John U. Kennedy Oubagaranadin and Z.V.P. Murthy If the initial adsorption rate is taken as h =
qt ; then when t approaches 0, h will become t
k2qe2. Now, Eq. (2.28) can be rearranged to obtain:
t 1 t qt h q e
(2.29)
2.2.4. Elovich Model The Elovich or Roginsky–Zeldovich equation (Low, 1960) is commonly used to describe the kinetics of chemisorption of gases onto heterogeneous solids. It is quite restricted as it only describes a limiting condition ultimately reached by the kinetic curve. The Elovich equation in its differential form is represented as,
dqt e exp( e qt ) dt
(2.30)
where, αe is the initial adsorption rate (mg/g-min) and βe is the desorption constant (g/mg) during any one experiment. Integration of Eq. (2.30), assuming the initial boundary condition qt = 0 at t = 0, gives
qt (1 / e ) ln(1 e e t )
(2.31)
To simplify the Elovich equation, Chien and Clayton (1980) assumed αeβet >> 1 and applied the boundary conditions qt = 0 at t = 0 and qt = qt at t = t, then the Eq. (2.31) becomes (Sparks, 1986):
qt (1 / e ) ln( e e ) (1 / e ) ln t
(2.32)
Thus, the constants can be obtained from the slope and intercept of the linearized plots of qt against ln(t).
2.2.5. Ritchie Model Ritchie kinetic model (Ritchie, 1977) was obtained assuming that the rate of adsorption depends only on the fraction of sites which are unoccupied at time t and is given as:
1 qt qe 1 r k r t where, βr and kr are constants.
(2.33)
Carbons and Clays for Heavy Metals Removal …
11
2.2.6. Intra-Particle Diffusion The overall adsorption process may be controlled either by one or more steps, e.g., filmdiffusion, pore-diffusion, surface-diffusion and adsorption on the pore surface, or a combination of more than one step. Besides adsorption at the outer surface of the adsorbent, there is also a possibility of intra-particle diffusion of the metal ions from the bulk of the outer surface into the pores of the adsorbent material, which is usually a slow process. The possibility of intra-particle diffusion can be studied using the intra-particle diffusion model (McKay et al. 1987; Weber and Morris, 1963) given by:
qt k ip t I
(2.34)
where, kip is the intra-particle diffusion rate constant and I is a constant that gives idea about the thickness of the boundary layer, i.e., larger the value of ‘I’ the greater is the boundary layer effect. When intra-particle diffusion is significant in controlling the kinetics of the adsorption process, the plot of qt vs. t yield straight lines passing through the origin and the slope gives the rate constant kip.
2.2.7. Film-Diffusion When the transport of the solute molecules from the liquid-phase to the solid-phase boundary plays a most significant role in adsorption, the liquid film-diffusion model (Boyd et al. 1947) can be applied, which is given as:
ln(1 F ) k fd t
(2.35)
where F is the fractional attainment of equilibrium (F = qt/qe), and kfd is the film diffusion rate constant. A linear plot of −ln(1−F) versus t with zero intercept would suggest that the kinetics of the adsorption process is primarily controlled by diffusion through the liquid film surrounding the solid adsorbent.
2.3. Thermodynamics Based on the fundamental thermodynamics concept, it is assumed that in an isolated system, energy cannot be gained or lost and the entropy change is the only driving force. In environmental engineering practice, both energy and entropy factors must be considered in order to determine which process will occur spontaneously. The Gibbs free energy change, ∆Gº, is the fundamental criterion of feasibility. Reactions occur spontaneously at a given temperature if ∆Gº is a negative quantity. The Gibbs free energy of an adsorption process, considering the adsorption equilibrium constant KL (which is same as Langmuir constant) is given by the following equation:
G RT ln K L
(2.36)
12
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
where T is the solution temperature (K) and R is the Universal gas constant (8.314 J/mol/K). The thermodynamic parameters, such as changes in Gibbs free energy (∆Gº), enthalpy (∆Hº) and entropy (∆Sº) were determined by using the equations given below (Smith and Van Ness, 1987; Ho and Ofomaja, 2005, 2006). Considering the relationship between free energy and equilibrium constant, change in equilibrium constant with temperature can be obtained in the differential form as follows:
d H o ln K L dT RT 2
(2.37)
After integration and rearrangement, the Eq.(2.37) becomes:
RT ln K L H TRY
(2.38)
where, Y is integration constant. Let ∆Sº = RY
(2.39)
and substituting ∆Gº will result into the following, ∆Gº = ∆Hº − T∆Sº
(2.40)
The slope and the intercept of the plot of ∆Gº versus T were used to determine the ∆Sº and ∆Hº values. Basically, the heat evolved during physical adsorption is of the same order of magnitude as the heat of condensation, i.e., 2.1–20.9 kJ/mol (Sag and Kutsal, 2000), while the heat of chemisorption generally falls in the range of 80–200 kJ/mol (Hayward and Trapnell, 1964).
3. ADSORBENTS FOR HEAVY METALS 3.1. Carbons Made from Bio-Materials Activated carbon has been the most popular and widely used adsorbent in wastewater treatment. In spite of its abundant use, activated carbon remains an expensive material since higher the quality of activated carbon, the greater the operation cost. Activated carbon also requires complexing agents to improve its removal performance for inorganic matters. Activated carbon is generally a good adsorbent for heavy metals in solutions. Nevertheless, it is essential to look for inexpensive sources from which activated carbon can be made. Wang et al. (2010) studied the adsorption of Cd(II) ions from aqueous solution by bamboo charcoal. The results showed that high pH (≥8.0) was favorable for the adsorption of Cd(II) ions. Higher initial Cd(II) concentrations led to lower removal percentages but higher adsorption capacity. As the adsorbent dose increased, the removal of Cd(II) increased, while
Carbons and Clays for Heavy Metals Removal …
13
the adsorption capacity decreased. Adsorption kinetics of Cd(II) ions onto bamboo charcoal was best described by the pseudo-second-order model. The adsorption of Cd(II) ions followed Langmuir isotherm, with a maximum adsorption capacity of 12.08 mg/g. This study demonstrated that bamboo charcoal could be used for the removal of Cd(II) ions from water treatment. Removal of Cr(VI) ions from aqueous solution was investigated by Owlad et al. (2010) using modified palm shell activated carbon. Low Molecular Weight Polyethyleneimine (LMWPEI) was used for impregnation purpose. The adsorption experiments were carried out in a batch system using potassium dichromate K2Cr2O7 as the source of Cr(VI) in the synthetic waste water and modified palm shell activated carbon as the adsorbent. The effects of pH, concentration of Cr(VI) and PEI loaded on activated carbon were studied. The adsorption data were found to fit well with the Freundlich isotherm model. This modified Palm shell activated carbon showed high adsorption capacity for chromium ions. Monser and Adhoum (2009) modified activated carbon with tartrazine and applied it for the removal of Pb(II), Cd(II) and Cr(III) ions at different pH values. The presence of tartrazine as modifier enhanced attractive electrostatic interactions between metal ions and carbon surface. The adsorption capacity for Pb(II), Cd(II) and Cr(III) ions improved with respect to non-modified carbon reaching a maximum of 140%. The adsorption capacity was found to be pH dependent for both modified and non-modified carbons with a greater adsorption at higher pH values except for Cr(III). The enhancement percent of Pb(II), Cd(II) and Cr(III) at different pH values varied from 28% to 140% with respect to non-modified carbon. Oubagaranadin and Murthy (2009a) prepared physically and chemically activated carbons using sal wood (Shorea robusta) sawdust by thermal process and using sulfuric acid as the activation agent and tested them to remove Pb(II) from aqueous solutions. Adsorption equilibrium studies were done at a pH of 4 and at the room temperature of 30ºC. It was found that the adsorption isotherms were favorable and chemically activated carbons were better than physically activated carbon in terms of adsorption capacity (≈ 7 mg/g for chemical activated carbons and 4 mg/g for physically activated carbon). The Freundlich adsorption model provided best-fit. The first-order irreversible unimolecular reaction model and the pseudo-second-order kinetic model provided good fit. Kinetic and film diffusion studies showed that the adsorption of lead(II) on the activated carbons tested were both intra-particle and film diffusion controlled. Tajar et al. (2009) studied adsorption of Cd(II) onto low-cost activated carbons derived from nut shells. Four kinds of activated carbons: prepared activated carbon (PAC), commercial activated carbon (CAC), and sulfurized PAC (SPAC) and sulfurized CAC (SCAC) were tested for the adsorption of Cd(II). With increasing pH, the adsorption of Cd(II) increased and maximum removal was observed to be 92.4% for SPAC at pH values greater than 8.0 (C0 = 100 mg/L). The H-type adsorption isotherms, obtained for the adsorbents, indicated a favorable process. Adsorption data better indicated Frendlich isotherm. The maximum adsorption capacities were 90.09, 104.17, 126.58 and 142.86 mg/g for CAC, PAC, SCAC and SPAC, respectively. Removal of Pb(II), Zn(II), Cu(II), and Cd(II) from aqueous solutions using activated carbon prepared from Phaseolus aureus hulls was studied by Rao et al. (2009). The removal of metal ions by the adsorbent was found to be pH dependent and the optimum pH values were 7.0, 8.0, 7.0 and 6.0 for Cu(II), Cd(II), Zn(II), and Pb(II), respectively. The maximum
14
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
adsorption capacity values for metal ions were 21.8 mg/g for Pb(II), 21.2 mg/g for Zn(II), 19.5 mg/g for Cu(II) and 15.7 mg/g for Cd(II). It was observed that the kinetic data followed the pseudo-second-order kinetic model. Li and Wang (2009) studied the removal of Pb(II) by low-cost activated carbon prepared from Spartina alterniflora by phosphoric acid activation. It was found that pH played a major role in the adsorption process. The maximum adsorption capacity for Pb(II) on S. alterniflora activated carbon calculated from Langmuir isotherm was about 99 mg/g. The optimum pH range for the removal of Pb(II) was 4.8-5.6. The Freundlich isotherm model best described the experimental data. The kinetic data fitted best to the pseudo-second-order model. Thermodynamic study showed that the adsorption was a spontaneous and exothermic in nature. The adsorption of Cu(II) ions from aqueous solutions by hazelnut shell activated carbon was studied in a batch adsorption system by Demirbas et al. (2009). Maximum adsorption of Cu(II) ions occurred at around pH 6. The adsorption kinetics was best described by the pseudo-second-order rate equation. The adsorption equilibrium data fitted best with the Langmuir isotherm and the monolayer adsorption capacity of Cu(II) ions was determined to be 58.27 mg/g at 323 K. The positive value of the thermodynamic parameter ΔH (18.77 kJ/mol) showed that the adsorption was endothermic. Acharya et al. (2009) studied the adsorption of Pb(II) on activated carbon prepared from Tamarind wood with zinc chloride activation. Adsorption studies were conducted in the range of 10–50 mg/L initial Pb(II) concentration and at temperature in the range of 10–50°C. The maximum adsorption capacity was observed as 43.85 mg/g. The rates of adsorption were found to confirm to pseudo-second-order kinetics with good correlation and the overall rate of Pb(II) uptake was found to be controlled by pore-diffusion, film-diffusion and particlediffusion, in the entire adsorption period. Thermodynamic parameters indicated that the sorption was feasible, spontaneous and endothermic in nature. The use of olive-waste cake, a by-product of the manufacture of olive oil, as a potential feedstock for the preparation of activated carbon was studied by Baccar et al. (2009). Chemical activation of this precursor, using phosphoric acid as dehydrating agent, was adopted. To enhance the adsorption capacity of the optimal activated carbon for heavy metals, a modification of the chemical characteristics of the adsorbent surface was performed, using KMnO4 as oxidant. The efficiency of this treatment was evaluated considering the adsorption of Cu(II) ions as a model for metallic species. The results also indicated that copper uptake capacity was enhanced by a factor of up to 3 for the permanganate-treated activated carbon. The suitability and performance of cattle-manure-compost based activated carbons in removing heavy metal ions from aqueous solution was studied by Zaini et al. (2009). The influence of ZnCl2 activation ratios and solution pH on the removal of Cu(II) and Pb(II) were studied. Batch adsorption technique was used to determine the metal-binding ability of activated carbons. It was found that the uptake of aqueous metal ions by activated carbons well described by Langmuir equation. The increase of surface area and mesopore ratio as a result of increasing activation ratios favored the removal of Cu(II), while activated carbon rich in acidic groups showed selective adsorption towards Pb(II). Activated carbons prepared from chestnut shells and grape-seeds were used as adsorbents for the removal of Cu (II) ions from aqueous solutions by Özçimen and Ersoy-Meriçboyu (2009). Adsorption experiments were performed by varying initial metal ion concentration, temperature and pH. Freundlich isotherm provided better fit to the equilibrium data. It was
Carbons and Clays for Heavy Metals Removal …
15
observed that the adsorption capacities of adsorbents increased with increasing temperature, pH and surface area. The adsorption ability of a powdered activated carbons derived from walnut shells was investigated by Zabihi et al. (2009), in an attempt to produce more economic and effective sorbents for the control of Hg(II) from industrial liquid streams. Carbonaceous adsorbents were prepared by chemical activation methods using ZnCl2 as activating reagent. It was shown that Hg(II) uptake decreased with increasing pH of the solution. The proper choice of preparation conditions resulted in microporous activated carbons with different BET surface areas of 780 (carbon A, 1:0.5 ZnCl2) and 803 (carbon B, 1:1 ZnCl2) m2/g BET surface area. The monolayer adsorption capacities of these particular adsorbents were obtained as 151.5 and 100.9 mg/g for carbons A and B, respectively. It was determined that Hg(II) adsorption followed Langmuir isotherm and pseudo-second-order kinetics. A report was presented on the feasibility of using agricultural waste and timber industry waste carbons by Bansal et al. (2009), to remove Cr(VI) from synthetic wastewater under different experimental conditions. Rice husk and saw dust were used as adsorbents after sulphuric acid treatment. Maximum metal removal was observed at pH 2.0. The efficiencies of rice husk carbon (RHC) and saw dust carbon (SDC) for Cr(VI) removal were 91.75% and 94.33%, respectively, for aqueous solutions (250 mg/L) at 20 g/L adsorbent dose. It was found that Langmuir, Dubinin-Radushkevich and Temkin models fitted well. The results revealed that Cr(VI) was adsorbed considerably on RHC and SDC, and it could be an economical method for its removal from aqueous systems. The surface areas of RHC and SDC were 1.12 and 1.16 m2/g, respectively. Pomegranate husk was converted into activated carbon and tested for its ability to remove hexavalent chromium from wastewater by Nemr (2009). The activated carbon was obtained from pomegranate husk by dehydration process using concentrated sulfuric acid. Batch equilibrium experiments exhibited that a maximum chromium uptake was obtained at pH 1.0. The maximum adsorption capacity for pomegranate husk activated carbon was 35.2 mg/g as calculated by Langmuir model. The ability of activated carbon to remove chromium from synthetic sea water, natural sea water and wastewater was investigated as well. This study showed that the removal of toxic chromium by activated carbon developed from pomegranate husk was promising. Activated charcoal was prepared from Melocanna baccifera (Poaceae) charcoal by chemical pretreatment in order to make better use of this biomass (Lalhruaitluanga et al., 2009). Batch experiments were conducted under varying range of pH (2.0–6.0), contact time (15–360 min) and metal ion concentrations (50–90 mg/L). The optimum conditions for lead biosorption are almost same for M. baccifera raw charcoal (MBRC) and M. baccifera activated charcoal (MBAC), viz., pH 5.0, contact time 120 min, adsorption capacity 10.66 mg/g and 53.76 mg/g. The biomass of MBAC was found to be more suitable than MBRC for the development of an efficient adsorbent for the removal of Pb(II) from aqueous solutions. FTIR analysis revealed that -OH, C-H bending, C=O stretching vibration and carbonyl functional groups were mainly responsible for Pb(II) biosorption. A study by Hsu et al. (2009) evaluated the removal of Cr(VI) from water by carbon derived from the burning of rice straw. Rice straw was burned in the air to obtain rice carbon (RC), and then the removal of Cr(VI) by RC was investigated under various pH and ionic strengths. This study revealed that Cr bound to RC was predominately in the trivalent form. The results showed that upon reacting with RC, Cr(VI) was reduced to Cr(III), which was
16
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
either adsorbed on RC or released back into solution. The extent and rate of Cr(VI) removal increased with decreasing solution pH because the Cr(VI) adsorption and the subsequent reduction of adsorbed Cr(VI) to Cr(III) both occur preferentially at low pH. The minimal effect of ionic strength on the rates of Cr(VI) removal and Cr(III) adsorption indicated specific interactions between Cr(VI)/Cr(III) and their surface binding sites on RC. These results suggest that rice straw-based carbon may be effectively used at low pH as a substitute for activated carbon for the treatment of Cr(VI) contaminated water. In a study by Ghosh (2009), fresh activated carbon (AC) and waste activated carbon (WAC) were pretreated by heating with sulfuric acid and nitric acid at high temperature to prepare different grades of adsorbents and evaluated their performance for Cr(VI) removal from aqueous solution. Batch adsorption equilibrium data followed both, Freuindlich and Langmuir isotherms. Maximum adsorption capacity of the selected adsorbents treated with sulfuric acid (WAC1) and nitric acid (WAC2), calculated from Langmuir isotherm were found to be 7.485 and 10.929 mg/g, respectively. Adsorption capacities for Cd(II) on indigenously prepared, steam activated, untreated, surfactant-modified carbon powder, from husk and pods of Moringa oleifera were investigated by Nadeem et al. (2009). The optimized conditions for all the experimental runs were pH 8.0, temperature 30°C, contact time 120 min, agitation speed 160 rpm, initial metal concentration 30 mg/L and adsorbent dosage 1.0 g/L. Maximum Cd(II) removal (98.0%) was observed when cetyltrimethyl ammonium bromide (CTAB), a cationic surfactant-treated carbon, was used as an adsorbent. The Cd(II) removal percentages for sodium dodecyl sulphate (SDS), anionic surfactant, Triton X-100 (non-ionic surfactant) treated and untreated powder activated carbons were found to be 95.60, 81.50 and 73.36%, respectively. SEM images and BET surface area, porosity and pore volume measurements revealed that surfactant-treated carbons had superior porosity and enhanced surface area than untreated carbons. The sorption data correlated better with the Langmuir adsorption isotherm. Oubagaranadin and Murthy (2009b) removed Cr(VI) from aqueous solutions of potassium dichromate by adsorption onto physically and chemically activated carbons derived from Zea mays (corn or maize cob), an agricultural waste product. Adsorption studies were done at the optimum pH of 2 and at the room temperature of 30ºC. The best fit to the equilibrium data was provided by the 3-parameter Fritz-Schluender model followed by the 2parameter Langmuir model. The adsorption isotherms were favorable and the adsorption on chemically activated carbons improved as the impregnation ratio was increased. Physically activated carbon showed better adsorption capacity (34 mg/g) than the chemically activated carbons (23.24, 27.1 and 33.4 mg/g). Kinetic modeling showed that the fractional power model provided the best fit. The adsorption of Cr(VI) on the activated carbons was filmdiffusion controlled. The use of an activated carbon developed from date palm seed wastes, generated in the jam industry, for removing toxic chromium from aqueous solution was investigated by Nemr et al. (2008). The activated carbon was obtained from date palm seed by dehydrating methods using concentrated sulfuric acid. A strong dependence of the adsorption capacity on pH was observed, the capacity increased as pH value decreased and the optimum pH value was 1.0. The adsorption process was fast and the equilibrium was reached within 180 min. The maximum removal was 100% for 75 mg/L of Cr(VI) concentration on 4 g/L carbon concentration and the maximum adsorption capacity was 120.48 mg/g. The Elovich equation
Carbons and Clays for Heavy Metals Removal …
17
and pseudo-second-order equation provided the greatest accuracy for the kinetic data, and Koble-Corrigan and Langmuir models the closest fits for the equilibrium data. A low-cost activated carbon prepared from Tamarind wood material by chemical activation with sulphuric acid for the adsorption of Pb(II) from dilute aqueous solution was studied by Singh et al. (2008). The activated carbon developed showed substantial capacity to adsorb Pb(II) from dilute aqueous solutions. The kinetic data were best fitted to the Lagergren pseudo-first-order and pseudo-second-order models. The isotherm equilibrium data were well fitted by the Langmuir and Freundlich models. The maximum removal of Pb(II) obtained was 97.95% (experimental) and 134.22 mg/g (from Langmuir isotherm model) at an initial concentration 40 mg/L, adsorbent dose 3 g/L and pH 6.5. This high uptake showed Tamarind wood activated carbon as a promising adsorbent for Pb(II). The use of a date-pit activated carbon and a commercially available activated carbon for the removal of trivalent aluminum from aqueous solutions were examined at various conditions by Al-Muhtaseb et al. (2008). In the acidic range of aluminum solubility (up to pH value of 4), both adsorbents exhibited maximum (almost equivalent) capacities for adsorbing aluminum at the pH value of 4. At low initial concentrations of aluminum and low pH, the uptake of aluminum using date-pit activated carbon was 0.305 mg/g, while that using commercial activated carbon was only 0.021 mg/g. However, the commercial activated carbon was more effective in adsorbing aluminum with high concentrations and low pH. Furthermore, date-pit activated carbon exhibited higher initial adsorption rates as compared to commercial one, which showed higher rates at longer periods of time. Nickel removal efficiency of sulphuric acid-treated Parthenium carbon (SWC) from simulated wastewater was investigated by Lata et al. (2008). Ni(II) removal was pHdependent and found to be maximum at pH 5.0. Both Freundlich and Langmuir adsorption isotherm models represented the experimental data satisfactorily. The monolayer adsorption capacities of SWC as obtained from Langmuir isotherm was found to be 17.24 mg/g. The pseudo-first-order model was less applicable than pseudo-second-order reaction model. The FTIR study indicated the presence of O-H, C-H, C=O and C-O groups in the adsorbent. Production of a modified carbon by heat treating bean husk (Phaseolus vulgaris) at 270 °C in Ar, followed by chemical activation using HNO3, was reported by ChávezGuerrero et al. (2008). Cd(II) sorption studies with this material were carried out at different concentrations and found that Cd(II) got effectively removed by the modified material obtained from bean husk (180 mg/g). An activated carbon prepared from olive stone was used for Cd(II) removal by Kula et al. (2008). Different activating agent (ZnCl2) amounts and adsorbent particle sizes were studied to optimize adsorbent surface area. The equilibrium time, optimum pH, adsorbent dosage were found to be 60 min, pH > 6 and 1.0 g/50 mL, respectively. The kinetic data supported pseudo-second-order model and intra-particle model. The activated carbons with 20% ZnCl2 solution was the best sample of the produced activated carbons from olive stone with the specific surface area of 790.25 m2/g. The results showed that the produced activated carbon from olive stone was an alternative low-cost adsorbent for removing Cd(II). Activated carbon prepared from hazelnut husks with zinc chloride activation at 973 K in nitrogen atmosphere was studied for adsorption of Cu(II) and Pb(II) by Imamoglu and Tekir (2008). BET surface area of the activated carbon was found as 1092 m2/g. The activated carbon exhibited good adsorption potential for copper and lead ions. The maximum
18
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
adsorption capacity of the adsorbent for Cu(II) and Pb(II) ions was calculated from the Langmuir isotherm and found to be 6.645 and 13.05 mg/g, respectively. The applicability of sulphurised activated carbon (SAC) as adsorbent for the effective removal of Co(II) from aqueous solutions was investigated by Krishnan and Anirudhan (2008). Bagasse pith, a sugarcane industry waste, was used for the synthesis of SAC. Maximum adsorption was observed in the pH range of 4.5–8.5. With an initial concentration of 50 and 100 mg/L of the adsorbate at pH 6.0, the percentage adsorptions were found to be 90.3 and 81.0%, respectively. SAC showed a high adsorption capacity for Co(II) removal when compared with laboratory and commercial grade activated carbons. The adsorption process obeyed Langmuir isotherm model. In a study by Demiral et al. (2008), activated carbon was prepared from olive bagasse by physical activation using steam. BET surface area of the activated carbon was determined as 718 m2/g. The maximum Cr(VI) adsorption yield was obtained at the initial pH of 2. The adsorption kinetics followed pseudo-second-order rate expression. Equilibrium results were analyzed by the Langmuir, Freundlich, Dubinin-Redushkevich, Temkin and Frumkin equations. Langmuir equation was found to fit the equilibrium data for Cr(VI) adsorption. Gerçel and Gerçel (2007) studied the adsorption of Pb(II) onto activated carbon prepared from renewable plant material, Euphorbia rigida. Adsorption data of Pb(II) onto activated carbon from E. rigida obeyed the Langmuir isotherm model. Maximum adsorption capacity of Pb(II) onto adsorbent was 279.72 mg/g at 40 °C. It was indicated that the adsorption of Pb(II) onto activated carbon from E. rigida could be described by the pseudo-second-order kinetic model and also followed the simple external-diffusion model for the initial 10 min and then by intra-particle diffusion model up to 50 min. A carbon rich adsorbent prepared from the reaction of sugar beet pulp with sulphuric acid and gas formed during carbonization process have been studied for Cr(VI) removal from aqueous solutions by Altundogan et al. (2007). The SO2 rich gas was shown to be an excellent Cr(VI) reductant. The equilibrium and kinetic studies were conducted by using the carbonaceous adsorbent derived from sugar beet pulp. Lower pH favored Cr(VI) adsorption, hence substantial Cr(VI) reduction was observed. Langmuir model best fitted the equilibrium isotherm data. The maximum adsorption capacity of chromium calculated from Langmuir isotherm was about 24 mg/g at 25 °C. The adsorption of Cr(VI) was endothermic and followed the pseudo-second-order rate kinetics. The sulphuric acid-carbonization was found to be economical particularly for chromium removal because the gas generated during carbonization exhibited good Cr(VI) reduction properties. In a study by Wilson et al. (2006) peanut shells were converted to activated carbons for use in adsorption of select metal ions; namely Cd(II), Cu(II), Pb(II), Ni(II) and Zn(II). Milled peanut shells were pyrolyzed in an inert atmosphere of nitrogen gas, and then activated with steam at different activation times. Following pyrolysis and activation, the carbons underwent air oxidation. The prepared carbons were evaluated for adsorption efficiency and these parameters were compared to the same parameters obtained from three commercial carbons, namely, DARCO 12 × 20, NORIT C GRAN and MINOTAUR. One of the peanut shell-based carbons had metal ion adsorption efficiency greater than two of the three commercial carbons but somewhat less than but close to MINOTAUR. This study demonstrated that the peanut shells can serve as a source for activated carbons with metal ion-removing potential and may serve as a replacement for coal-based commercial carbons in applications that warrant their use.
Carbons and Clays for Heavy Metals Removal …
19
The performance of a commercially available palm shell based activated carbon to remove Pb(II) from aqueous solutions by adsorption was evaluated by Issabayeva et al. (2006). The adsorption experiments were carried out at pH 3.0 and 5.0. Palm shell activated carbon showed high adsorption capacity for Pb(II), especially at pH 5 with an ultimate uptake of 95.2 mg/g. This high uptake showed palm shell activated carbon as a promising adsorbent. Removal and recovery of chromium were carried out by using low-cost activated carbon made from sugar industry waste (Fahim et al., 2006). Three types of activated carbons, viz., C1 (the waste generated from sugar industry) and the others C2, C3 (commercial granular activated carbons) were used. The effect of pH, particle size and type of adsorbent on the adsorption isotherm of Cr(III) were studied in batch system. The sorption data fitted well with Langmuir adsorption model. The efficiencies of activated carbons for the removal of Cr(III) were found to be 98.86, 98.6 and 93 % for C1, C2 and C3, respectively. The order of selectivity was C1 > C2 > C3 for removal of Cr(III) from tannery wastewater. Carbon “C1” of the highest surface area (520.66 m2/g) had the highest adsorptive capacity for the removal of Cr(III). The results revealed that the trivalent chromium was significantly adsorbed on activated carbon collected from sugar industry waste. Kannan and Rengasamy (2005) studied the removal of Cd(II) from aqueous solutions by adsorption on commercial activated carbon (CAC) and chemically prepared activated carbons (CPACs) from raw materials such as straw, saw dust and datesnut. The percentage removal increased with decrease in initial concentration and particle size of CPACs and an increase in contact time, dose and initial pH of the solution. The kinetics of adsorption was found to be first order with intra-particle diffusion as one of the rate determining steps. Results of the studies on adsorption of Cd(II) ions from simulated wastewater were compared with that of CAC and Tulsion CXO-9(H), a commercial ion exchange resin / cationic resin (CR). Straw carbon showed the maximum adsorption capacity towards Cd(II). Granular activated carbon (GAC) was treated chemically with potassium bromate for surface modification and its adsorption capacity was investigated with nickel ions by Satapathy and Natarajan (2006). There was an increase in the adsorption capacity of the modified carbon by 90–95% in comparison with the raw granular activated carbon towards nickel ions. Potassium bromate oxidation treatment was employed for a period of about 30 min initially followed by 60 min and the oxidized carbons were adsorbed with nickel ions. Metal adsorption characteristics of as received and modified activated carbons were measured in batch experiments. Equilibrium data fitted well with Langmuir model which indicated monolayer adsorption. Effects of pH of initial solution, time of oxidation and mode of treatment on the adsorption process were studied. Experimental results showed that metal uptake increased with an increase in pH and oxidation time. An efficient adsorption process was reported for the decontamination of Cr(III) from tannery effluents by Mohan et al. (2006). A low cost activated carbon (ATFAC) was prepared from coconut shell fibers and utilized for Cr(III) removal from water/wastewater. A commercially available activated carbon fabric cloth (ACF) was also studied for comparative evaluation. The Langmuir model best fitted the equilibrium isotherm data. The maximum adsorption capacities of ATFAC and ACF at 25 °C were 12.2 and 39.56 mg/g, respectively. Cr(III) adsorption increased with an increase in temperature (at 10 °C, ATFAC: 10.97 mg/g, ACF: 36.05 mg/g; at 40 °C, ATFAC: 16.10 mg/g, ACF: 40.29 mg/g). The adsorption of Cr(III) followed the pseudo-second-order rate kinetics. The sorption capacities of ATFAC
20
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
and ACF were comparable to many other adsorbents / carbons / biosorbents utilized for the removal of trivalent chromium from water/wastewater. Activated carbon prepared from Ceiba pentandra hulls, an agricultural solid waste byproduct, for the removal of copper and cadmium from aqueous solutions was studied by Rao et al. (2006). The adsorbent exhibited good sorption potential for copper and cadmium at pH 6.0. The C=O and S=O functional groups present on the carbon surface were the adsorption sites to remove metal ions from solution. The maximum adsorption capacity of Cu(II) and Cd(II) was calculated from Langmuir isotherm and found to be 20.8 and 19.5 mg/g, respectively. Desorption studies were carried out using dilute HCl and the effect of HCl concentration on desorption was also studied. Maximum desorption of 90% for Cu(II) and 88% for Cd(II) occurred with 0.2 M HCl. Apricot stones were carbonized and activated after treatment with sulphuric acid (1:1) at 200 °C for 24 h by Kobya et al. (2005). The ability of the activated carbon to remove Ni(II), Co(II), Cd(II), Cu(II), Pb(II), Cr(III) and Cr(VI) ions from aqueous solutions by adsorption was investigated. Batch adsorption experiments were conducted to observe the effect of pH (1–6) on the activated carbon. The adsorption of these metals was found to be dependent on solution pH. Highest adsorption occurred at pH 1-2 for Cr(VI) and pH 3-6 for the rest of the metal ions, respectively. Adsorption capacities for the metal ions were obtained in the order of Cr(VI) > Cd(II) > Co(II) > Cr(III) > Ni(II) > Cu(II) > Pb(II) for the activated carbon prepared from apricot stone. Adsorption capacity of Cr(VI) onto Hevea brasilinesis (rubber wood) sawdust activated carbon was investigated in a batch system by considering the effects of various parameters like contact time, initial concentration, pH and temperature by Karthikeyan et al., 2005. Cr(VI) removal was found to be maximum at pH 2.0. Increase in adsorption capacity with increase in temperature indicated that the adsorption reaction was endothermic. Pseudosecond-order model was found to explain the kinetics of Cr(VI) adsorption most effectively. Intraparticle diffusion studies at different temperatures show that the mechanism of adsorption is mainly dependent on diffusion. Langmuir isotherm showed better fit than Freundlich and Temkin isotherms in the temperature range studied. The results showed that the rubber wood sawdust activated carbon can be efficiently used for the treatment of wastewaters containing chromium as a low cost alternative. Removal of Pb(II) from aqueous solutions by adsorption onto coconut-shell carbon was investigated by Sekar et al. (2004). Adsorption of Pb(II) was strongly affected by pH. The coconut-shell carbon (CC) exhibited the highest lead adsorption capacity at pH 4.5. The equilibrium data fitted well to the Langmuir model. At pH 4.5, the maximum lead adsorption capacity of CC estimated with the Langmuir model was 26.50 mg/g. The thermodynamics of Pb(II) on CC indicated spontaneous and endothermic nature of the adsorption. Quantitative desorption of Pb(II) from CC was found to be 75% which facilitated the adsorption of metal by ion exchange. In a study, the technical feasibility of coconut shell charcoal (CSC) and commercial activated carbon (CAC) for Cr(VI) removal was investigated in batch studies using synthetic electroplating wastewater (Babel and Kurniawan, 2004). Both the granular adsorbents were made up of coconut shells (Cocos nucifera L.). Surface modifications of CSC and CAC with chitosan and/or oxidizing agents, such as sulfuric acid and nitric acid, respectively, were also conducted to improve removal performance. The adsorbents chemically modified with an oxidizing agent demonstrated better Cr(VI) removal capabilities than as-received adsorbents
Carbons and Clays for Heavy Metals Removal …
21
in terms of adsorption rate. Both CSC and CAC, which were oxidized with nitric acid, had higher Cr(VI) adsorption capacities (CSC: 10.88, CAC: 15.47 mg/g) than those oxidized with sulfuric acid (CSC: 4.05, CAC: 8.94 mg/g) and non-treated CSC coated with chitosan (CSCCC: 3.65 mg/g), respectively, suggesting that surface modification of a carbon adsorbent with a strong oxidizing agent generated more adsorption sites on their solid surface for metal adsorption. Hasar (2003) prepared activated carbon from almond husk by activating without (MACI) and with (MAC-II) H2SO4 at different temperatures. The ability of the activated carbon to remove Ni(II) from aqueous solutions by adsorption has been investigated under several conditions such as pH, carbonization temperature of husk, initial concentration of metal ions, contact time, and adsorbent concentration. Optimal conditions were pH 5.0, the carbonization temperature of 700 °C, 50 min of contact time and adsorbent concentration of 5 g/L. The results indicated that the effective uptake of Ni(II) ions was obtained by activating the carbon, prepared from almond husk at 700 °C, through the addition of H2SO4. The removal of Ni(II) was found to be 97.8% at initial concentration of 25 mg/L and the adsorbent concentration of 5 g/L. When the adsorbent concentration was increased up to 40 g/L, the adsorption capacity decreased from 4.89 to 0.616 mg/g for MAC-II. In the isotherm studies, the experimental adsorption data fitted reasonably well to Langmuir isotherm for both MAC-I and MAC-II. The use of low-cost activated carbon derived from bagasse was investigated by Mohan and Singh, (2002) for the removal of Cd(II) and Zn(II). The uptake of Cd(II) was found to be slightly greater than that of Zn(II) and the adsorption capacity increased with increase in temperature. The adsorption equilibrium data were better fitted by the Freundlich isotherm as compared to Langmuir in both the single- and multi-component systems. The adsorption occurred through a film diffusion mechanism at low as well as at higher concentrations. Activated carbon (AC) prepared from waste Parthenium was used to eliminate Ni(II) from aqueous solution by adsorption (Kadirvelu et al., 2002). The adsorption capacity calculated from the Langmuir isotherm was 54.35 mg Ni(II)/g of AC at initial pH of 5.0 and 20°C, for the particle size 250-500 μm. Increase in pH from 2 to 10 increased percent removal of the metal ions. The regeneration of Ni(II)-saturated carbon by HCl indicated an adsorption mechanism by ion-exchange between metal ions and H+ ions on the AC surfaces. Quantitative recovery of Ni(II) was possible with HCl. Activated carbon prepared from coconut tree sawdust was used as an adsorbent for the removal of Cr(VI) from aqueous solution by Selvi et al. (2001). Adsorption capacity was calculated from the Langmuir isotherm and was 3.46 mg/g at an initial pH of 3.0 for the particle size 125-250 μm. The adsorption of Cr(VI) was pH dependent and maximum removal was observed in the acidic pH range. A summary of carbons made from different starting materials and their adsorption capacities for different heavy metal ions is given in Table 3.1.
3.2. Clays Clays are one of the prospective low cost alternatives to activated carbons as adsorbents for the heavy metals removal. The clays sorption capabilities come from their high surface area (up to 800 m2/g) and exchange capacities (Cadena et al., 1990). The negative charge on the structure of clay minerals gives clay the capability to attract metal ions. There are three
22
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
basic species of clay, viz., smectites (such as montmorillonite), kaolinite, and micas; out of which montmorillonite has the highest cation exchange capacity. Therefore, a number of studies have been conducted using clays to show their effectiveness for removing metal ions. Table 3.1. Activated carbon adsorbents for heavy metals from solutions Source material for activated carbon Bamboo Shorea robusta
Waste activated carbon (WAC)
Adsorption capacity,Reference qm (mg/g) 12.08 Wang et al., 2010 PAC: 4.0 Oubagaranadin and CACs : ≈ 7.0 Murthy, 2009a Cd(II) CAC: 90.09 Tajar et al., 2009 PAC: 104.17 SCAC: 126.58 SPAC: 142.86 Pb(II), Zn(II), 21.8, 21.2, 19.5, 15.7 Rao et al., 2009 Cu(II), Cd(II) Pb(II) 99 Li and Wang, 2009 Cu(II) 58.27 Demirbas et al., 2009 Pb(II) 43.85 Acharya et al., 2009 Hg(II) A: 151.5; B:100.9 Zabihi et al., 2009 Cr(VI) 35.2 Nemr, 2009 Pb(II) MBRC: 10.66 Lalhruaitluanga et al., MBAC: 53.76 2009 Cr(VI) WAC1: 7.48 Ghosh, 2009 WAC2: 10.93
Zea Mays
Cr(VI)
Date palm seed wastes Date-pit
Cr(VI) Al(III)
PAC: 34 CAC1: 23.24 CAC2: 27.1 CAC3: 33.4 120.48 0.305
Parthenium Bean husk (Phaseolus vulgaris) Euphorbia rigida Sugar beet pulp Palm shell Coconut shell fibers Ceiba pentandra hulls Coconut-shell Coconut shell
Ni(II) Cd(II)
17.24 180
Pb(II) Cr(VI) Pb(II) Cr(III) Cu(II), Cd(II) Pb(II) Cr(VI)
279.72 24 95.2 12.2 20.8, 19.5 26.5 10.88
Parthenium Coconut tree sawdust
Ni(II) Cr(VI)
54.35 3.46
Nut shells
Phaseolus aureus hulls Spartina alterniflora Hazelnut shell Tamarind wood Walnut shells Pomegranate husk Melocanna baccifera
Adsorbate metal ion Cd(II) Pb(II)
Oubagaranadin and Murthy, 2009b
Nemr et al., 2008 Al-Muhtaseb et al., 2008 Lata et al., 2008 Chávez-Guerrero et al., 2008 Gerçel and Gerçel, 2007 Altundogan et al., 2007 Issabayeva et al., 2006 Mohan et al., 2006 Rao et al., 2006 Sekar et al., 2004 Babel and Kurniawan, 2004 Kadirvelu et al., 2002 Selvi et al., 2001
Vieira et al. (2010) studied the adsorption of nickel on calcined Bofe bentonite clay. The influence of parameters such as pH, amount of adsorbent, adsorbate concentration and temperature was investigated. The kinetics data were better represented by the second-order model. The Bofe clay removed nickel with a maximum adsorption capacity of 1.91 mg/g of clay (20°C, pH 5.3) and that the thermodynamic data indicated that the adsorption reaction was spontaneous and exothermic. The Langmuir model provided the best fit for sorption isotherms.
Carbons and Clays for Heavy Metals Removal …
23
Ghorbel-Abid et al. (2009) characterized local clay from Jebel Chakir (Tunisia, North Africa). The clay was basically a smectite with a small proportion of kaolinite. The adsorption properties of the natural clay and the Na-purified clay in a chromium rich aqueous solution was studied by batch technique. The amount of adsorbed chromium ions was determined for the adsorption systems as a function of contact time, pH, adsorbent, and metal ion concentration. The results showed that the uptake of Cr (III) at pH 4, by the purified clay was very rapid. The quantity removed from the solution reached a maximum value at 15 min after mixing, and 1 h for the natural clay, although the latter removes greater quantities of Cr(III) ions compared to the Na-purified clay. The amounts adsorbed by the natural clay were about 117.5 mg of Cr(III)/g of clay and 61.4 mg/g with the Na-purified clay. Moreover, the results showed that the adsorption behavior of both the clays depended highly on the pH. Adsorption increased with the pH of the suspension in the range of 3-5.3. The pH was limited to values equal or less than 5.3 because of the precipitation of the hydroxide chromium at higher pH. The equilibrium data well fitted to the linearized Freundlich isotherm for the natural clay and Langmuir model for the Na-purified clay. Three types of Saudi Arabian clays, viz., Tabuk, Baha, and Khaiber; were tested for their abilities to adsorb Pb(II) from wastewater by Al-Jlil and Alsewailem (2009). The clays were treated with hydrochloric acid to activate adsorption sites within clay particles. Untreated Tabuk clay had the largest adsorption capacity for Pb(II), about 30 mg/g, in comparison with those of Baha and Khaiber clays. Least adsorption was observed with Khaiber clay, about 10 mg/g, which was attributed to the prior existence of lead within the clay. Adsorption of the acid-activated clays was not enhanced compared to those of untreated clays. The Langmuir model described the experimental data for all untreated clays, while the Freundlich model described the experimental data of untreated Khaiber clay and treated Baha clay. The results showed that the Tabuk clay could be utilized as a cost-effective and efficient adsorbent for removing heavy metals from wastewater in Saudi Arabia. Modified kaolinite clay with 25% (w/w) aluminium sulphate and unmodified kaolin were investigated as adsorbents to remove Pb(II) from aqueous solution by Jiang et al., 2009. The results showed that the amount of Pb(II) adsorbed onto modified kaolin (20 mg/g) was more than 4.5 times than that adsorbed onto unmodified kaolin (4.2 mg/g) under optimized conditions. It was observed that the data from both the adsorbents fitted well to the Langmuir isotherm. The kinetic adsorption of modified and unmodified kaolinite clay fitted well to the pseudo-second-order kinetic model. Experiments with real wastewater showed that higher amount of Pb(II) (the concentration reduced from 178 to 27.5 mg/L) and other metal ions were removed by modified kaolinite clay as compared with unmodified adsorbent (the concentration reduced from 178 to 168 mg/L). In a work by Wang et al. (2009), removal of Pb(II) from aqueous solution by adsorption onto Na-bentonite was reported under ambient conditions as a function of shaking time, pH, ionic strength, Na-bentonite content and temperature using batch technique. The kinetic adsorption was well described by the pseudo-second-order rate equation. The adsorption of Pb(II) on Na-bentonite was strongly dependent on pH. The Langmuir model fitted the adsorption isotherm very well. The thermodynamic parameters suggested that the adsorption of Pb(II) was endothermic and spontaneous. At low pH, the adsorption of Pb(II) was dominated by outer-sphere surface complexation and ion exchange with Na+/H+ on Nabentonite surfaces, whereas inner-sphere surface complexation was the main adsorption mechanism at high pH.
24
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
A hectorite (H) clay sample was modified with 2-mercaptobenzimidazole using homogeneous and heterogeneous routes by Guerra et al. (2009). Both modification methodologies resulted in similar products, named HHOM and HHET, respectively. The effect of two variables (contact time and metal concentration) was studied using batch technique at room temperature and pH 2.0. After achieving the best conditions for Cr(VI) adsorption, isotherms of this adsorbate on using the chosen adsorbents were obtained, which were fitted to non-linear Sips isotherm model. The maximum number of moles adsorbed was determined to be 11.63, 12.85 and 14.01 mmol/g for H, HHOM and HHET, respectively, reflecting the maximum adsorption order of HHET > HHOM > H. Batch sorption experiments were conducted with cadmium and lead ions at low equilibrium concentrations in 0.01 M of NaNO3 onto Petra clay in single component systems by Baker (2009). The equilibrium isotherms were determined at pH 6 under constant ionic strength and at different temperature. From the Langmuir isotherm, the equilibrium adsorption capacity for Cd(II) was found to be 74.074 to 144.927 mg/g and that for Pb(II) was 83.333 to 263.158 mg/g. The results showed that Petra clay, which was mainly composed of 20% of kaolinite and 55% of calcium montmorillomite, exhibited higher selectivity for Pb(II), whereas its selectivity for Cd(II) was often lower at all concentrations studied. From the R2 values for different isotherm models it was found that the sorption was good for the two metal ions and good correlation confirmed the formation of a monolayer of Cd(II) and Pb(II) on the surface of the clay. Isotherms analysis showed that the binding for these metal ions with Petra clay minerals was physisorption and the process was endothermic. Oubagaranadin and Murthy (2009c) studied the removal of Pb(II) from aqueous solution by adsorption on a montmorillonite-illite type of clay (MIC) collected from the Gulbarga district of Karnataka, India. Batch adsorption equilibrium data were determined with different initial Pb(II) concentrations (100, 150, and 200 ppm) at pH 4 and 37 °C, and the data were tested with isotherm models. The three-parameter Freundlich-Langmuir model gave the best fit to the equilibrium data. However, as the initial Pb(II) concentration was increased (150 and 200 ppm), then multi-layer adsorption was observed. The maximum monolayer adsorption capacity of the clay was determined to be ~ 52 mg/g. Kinetic studies indicated that the rate of adsorption of Pb(II) on the clay followed a second-order rate mechanism, with decreasing rate constant values of 0.1097, 0.0571, and 0.0022 g/(mg min) as the initial Pb(II) concentration was increased in the order of 100, 150, and 200 ppm, respectively. The value of the Freundlich constant (n) in the range of 2.5-4.6 indicated that MIC was a good adsorbent of divalent lead. At a higher initial Pb(II) concentration (200 ppm), the adsorption process was determined to be film-diffusion controlled, with a rate of 0.051 min-1. The mean values of the thermodynamic parameters showed that the adsorption process was endothermic, thermodynamically favorable, and spontaneous. The proposed two-stage adsorber system has reduced the clay dose by 8.5%, as compared to that of a single-stage adsorption system. In another work by Oubagaranadin and Murthy (2010), the natural montmorillonite-illite clay was activated with sulfuric acid and used for lead(II) removal. Raw clay disintegrated on acid activation and showed a particle size distribution. The montmorillonite and illite phases in the raw clay disappeared on acid activation and the activated clay, showed with sodiumaluminum-silicate and beidellite phases apart from quartz (low) phase. When tested for adsorption of Pb(II) in aqueous solutions, the acid-activated clay showed about 50% increased adsorption than raw clay. Sips adsorption isotherm and pseudo-second-order kinetic models were found to be best for the batch adsorption data. Kinetic studies showed the
Carbons and Clays for Heavy Metals Removal …
25
existence of film diffusion and intraparticle diffusion. A two-stage batch adsorber was designed for the removal of Pb(II) from aqueous solutions. There was about 63% increase in the monolayer adsorption capacity of the clay adsorbent due to acid activation. From the twostage batch adsorption system proposed using the experimental data, it was observed that the two-stage system reduced the adsorbent dose by about 14 and 30% of raw and activated clay, respectively, when compared with that of single-stage adsorption system. Adsorption of Cu(II) ions on a zeolite, clay and diatomite from Serbia was studied by Ńljivić et al. (2009), at different pH. The amounts of Cu(II) removed from the solution increased with increasing initial pH, reaching nearly 100% at pH > 7, due to precipitation of Cu(OH)2. Relatively constant final pH values and less significant increase of Cu(II) uptake was observed in the initial pH range 4–6, which have pointed out the role of buffering properties of investigated adsorbent materials. The maximum adsorption capacities decreased in the order of zeolite (0.128 mmol/g) > clay (0.096 mmol/g) > diatomite (0.047 mmol/g). The Langmuir isotherm gave the best fit. Ion exchange of exchangeable cations and protons were identified as main adsorption mechanisms. Removal of Cr(III) and Cr(VI) from aqueous solutions by white, yellow and red sands from the United Arab Emirates, as low cost abundant adsorbents, was investigated by Khamis et al. (2009). The effect of contact time, pH, temperature, metal concentration and sand dosage were studied. The optimal pH for adsorption was 5.0 for Cr(III) and 2.0 for Cr(VI). The optimal adsorption time for both ions was 3 h. Even at the optimal pH, adsorption of Cr(VI) on all sand forms was very low (removal ≤10%) and could not be fitted to any of the common isotherms. While at pH 5.0, Cr(VI) was not at all adsorbed and Cr(III) was totally removed. Adsorption of Cr(III) by the three sand forms obeyed Lagergren first-order kinetics. For Cr(III), the Langmuir isotherm gave best fit for adsorption. At 25 °C, the maximum mass of Cr(III) removed per gram of sand was 62.5, 9.80 and 2.38 (mg/g) for white, yellow and red sands, respectively. ΔH° was 14.5, 51.2 and 45.8 kJ/mol and ΔS° was 24.0, 136 and 111 J /K/mol for adsorption on white, yellow and red sands, respectively. Unuabonah et al. (2008a) studied the adsorption behavior of a polyvinyl alcohol modified (PVA-modified) kaolinite clay. Modification of kaolinite clay with PVA increased its adsorption capacity for 300 mg/L Pb(II) and Cd(II) by a factor of about 6, i.e., from 4.5 mg/g to 36.23 mg/g and from 4.38 mg/g to 29.85 mg/g, respectively, at 298 K. Binary mixtures of Pb(II) and Cd(II) decreased the adsorption capacity of unmodified kaolinite clay for Pb(II) by 26.3% and for Cd(II) by 0.07%, respectively. For PVA-modified kaolinite clay, the reductions were up to 50.9% and 58.5% for Pb(II) and Cd(II), respectively. The adsorption data of Pb(II) and Cd(II) onto both unmodified and PVA-modified kaolinite clay adsorbents were found to fit the pseudo-second-order kinetic model, indicating that adsorption on both the surfaces was mainly by chemisorption. Kaolinite clay obtained from Ubulu-Ukwu in Nigeria was modified with sodium tetraborate (NTB) to obtain NTB-modified kaolinite clay by Unuabonah et al. (2008b). Modification with sodium tetraborate reagent increased the adsorption capacity of kaolinite clay from 16.16 mg/g to 42.92 mg/g for Pb(II) and 10.75 mg/g to 44.05 mg/g for Cd(II) at 298 K. Increasing temperature was found to increase the adsorption of both the metals onto both the adsorbents suggesting endothermic adsorption. The simultaneous presence of electrolyte in aqueous solution with Pb(II) and Cd(II) was found to decrease the adsorption capacity of NTB-modified adsorbent for Pb(II) and Cd(II). The thermodynamic calculations for the modified kaolinite clay sample indicated an endothermic nature of adsorption and an
26
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
increase in entropy as a result of adsorption of Pb(II) and Cd(II). The small positive values of free energy change indicated that the adsorption of Pb(II) and Cd(II) onto the modified adsorbent may require some small amount of energy to make it more feasible. Modeling equilibrium adsorption data suggested that NTB-modified adsorbent sample had homogeneous adsorption sites and fitted well with Langmuir model. NTB-modified kaolinite clay sample showed good potentials as a low-cost adsorbent for the adsorption of Pb(II) and Cd(II) from aqueous solutions. Adsorption of Cu(II) by raw bentonite (RB) and acid-activated bentonite (AAB) samples was investigated by Eren and Afsin (2008) as a function of initial Cu(II) concentration, solution pH, ionic strength, temperature, the competitive and complexation effects of ligands (Cl−, SO42−, PO43−). Langmuir monolayer adsorption capacity of the RB (42.41 mg/g) was found to be greater than that of the AAB (32.17 mg/g). The spontaneity of the adsorption process was established by decrease in ΔG which varied from −0.34 to −0.71 kJ/mol (RB), −1.13 to −1.49 kJ/mol (AAB) in the temperature range of 303-313 K. Infrared (IR) spectra of the bentonite samples showed that the positions and shapes of the fundamental vibrations of the OH and Si-O groups were influenced by the adsorbed Cu(II) cations. Differential thermal analysis (DTA) results showed that adsorbed Cu(II) cations have a great effect on the thermal behavior of the bentonite samples. The X-ray diffraction (XRD) spectra indicated that the Cu(II) adsorption onto the bentonite samples led to changes in unit cell dimensions and symmetry of the parent bentonites. Eren (2008) reported the adsorption of Cu(II) from aqueous solution on modified Unye bentonite. Adsorption of Cu(II) by manganese oxide modified bentonite (MMB) sample was investigated as a function of the initial Cu(II) concentration, solution pH, ionic strength, temperature and inorganic ligands (Cl−, SO42−, HPO42−). The adsorption properties of raw bentonite were further improved by modification with manganese oxide. Langmuir monolayer adsorption capacity of the MMB (105.38 mg/g) was found to be greater than that of the raw bentonite (42.41 mg/g). The spontaneity of the adsorption process was established by decrease in ΔG which varied from −4.68 to −5.10 kJ/mol in temperature range of 303– 313 K. The high performance exhibited by MMB was attributed to the increased surface area and higher negative surface charge acquired after modification. The adsorption of Pb(II) onto Tunisian smectite-rich clay in aqueous solution was studied in a batch system by Chaari et al. (2008). In this study, four samples of clay (AYD, AYDh, AYDs, AYDc) were used. The AYD was raw clay. AYDh and AYDs correspond to AYD activated by 2.5 mol/L hydrochloric acid and 2.5 mol/L sulphuric acid, respectively. AYDc corresponds to AYD calcined at different temperatures (100, 200, 300, 400, 500 and 600 °C). Preliminary adsorption tests showed that sulphuric acid and hydrochloric acid activation of raw AYD clay enhanced its adsorption capacity for Pb(II). However, the uptake of Pb(II) by AYDs was very high compared to that of AYDh. This fact was attributed to the greater solubility of clay minerals in sulphuric acid compared to hydrochloric acid. Thermo activation of AYD clay reduced the Pb(II) uptake as soon as calcination temperature reaches 200 °C. Kinetic experiments showed that the sorption of lead ions on AYDs was very fast and the equilibrium was practically reached after only 20 min. The results also revealed that the adsorption of lead increased with increase in the solution pH from 1 to 4.5 and then decreased slightly between pH 4.5 and 6, and rapidly at pH 6.5 due to the precipitation of Pb(II) ions. The equilibrium data were analyzed using Langmuir isotherm model. The maximum adsorption capacity increased from 25 to 25.44 mg/g with increasing temperature from 25 to
Carbons and Clays for Heavy Metals Removal …
27
40 °C. It was observed that sulphuric acid activated clay was more efficient than physically activated clay. Adsorption of Cr(VI) onto spent activated clay (SAC), a waste produced from an edible oil refinery company, was investigated for its beneficial use in wastewater treatment by Weng et al. (2008). After pressure steam treatment, SAC was used as an adsorbent. The adsorption kinetic data were analyzed and fitted well with pseudo-first-order equation and the rate of removal was found to speed up with decreasing pH and increasing temperature. The maximum adsorption capacities for Cr(VI) were ranged from 0.743 to 1.422 mg/g for temperature between 4 and 40 °C under a condition of pH 2.0. The studies conducted show the process of Cr(VI) removal to be spontaneous at high temperature and endothermic in nature. Kaolinite and montmorillonite were used as adsorbents for Fe(III), Co(II) and Ni(II) in aqueous medium by Bhattacharyya and Gupta (2008). The effect of different variables, namely, concentration of metal ions, amount of clay adsorbents, pH, time and temperature of interaction was investigated. Adsorption increased with pH till precipitation of insoluble hydroxides became dominant. The processes conformed to second-order kinetics. Montmorillonite had a much higher adsorption capacity for the metal ions with the Langmuir monolayer capacity of 28.4 to 28.9 mg/g compared to that of 10.4 to 11.2 mg/g for kaolinite. All the interactions were exothermic except those between Co(II) and kaolinite. The adsorption processes were accompanied by an appreciable decrease in Gibbs energy. Both kaolinite and montmorillonite were observed to be suitable for treating water contaminated with Fe(III), Co(II) and Ni(II). Argun (2008) described the removal of Ni(II) ions from aqueous solutions using clinoptilolite. The effect of clinoptilolite level, contact time, and pH were determined. Different isotherms were also obtained using concentrations of Ni(II) ions ranging from 0.1 to 100 mg/L. The ion-exchange process followed second-order kinetics and the Langmuir isotherm. The work revealed that the ion-exchange process was spontaneous and exothermic under natural conditions. The maximum removal efficiency obtained was 93.6% at pH 7 and with a 45 min contact time (for 25 mg/L initial concentration and a 15 g/L solid-to-liquid ratio). The use of bentonite for the removal of Pb(II) from aqueous solutions for different contact times, pH of suspension, and initial concentration of lead and particle sizes of absorbent was investigated by Zhu et al. (2008). Batch adsorption kinetic experiments revealed that the adsorption of Pb(II) onto bentonite involved fast and slow processes. The adsorption mechanisms in the lead/bentonite system followed pseudo-second-order kinetics with a significant contribution of film-diffusion. The Langmuir model represented the adsorption process. The maximum adsorption capacity of Pb(II) onto natural bentonite was 78.82 mg/g. Çoruh (2008) investigated the effects of conditioning with NaCl and HCl solutions on the removal of Zn(II) from aqueous solutions using natural clinoptilolite collected from ManisaGördes region of Turkey. The clinoptilolite sample was used in four different forms, which consisted of one unconditioned (NC) and three conditioned (CC1, CC2 and CC3). The results clearly showed that the conditioning improved both the exchange capacity and the removal efficiency. It was found that the highest removal efficiency was obtained with CC2 sample. Adsorption isotherm of Zn(II) was best modeled by the Langmuir equation. The maximum adsorption capacities for Zn(II) shown by NC, CC1, CC2 and CC3 samples were 21.2, 20.8,
28
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
22.2 and 17.9 mg/g, respectively. Results indicate a significant potential for the natural and conditioned clinoptilolites as an adsorbent/ion-exchange material for heavy metal removal. Trivalent chromium was removed from synthetic wastewater using low-cost diatomite in batch and continuous systems by Gürü et al. (2008). In batch system, four different sizes and five different amounts of adsorbent were used. Langmuir adsorption capacities were found to be 28.1, 26.5 and 21.8 mg Cr(III)/g diatomite at 15, 30 and 45 °C, respectively. Adsorption process was exothermic in nature. The kinetic data showed that the pseudo-second-order equation was more appropriate, which indicated that the intra-particle diffusion is the ratelimiting factor. Laboratory grade Fuller‟s earth (FE) was used as an adsorbent in a work by Oubagaranadin et al. (2007) to remove mercury from aqueous solutions. For the purpose of comparison, simultaneous experiments using laboratory grade activated carbon (AC) was also done. Isotherms such as Freundlich, Langmuir, Dubinin–Radushkevich, Temkin, HarkinsJura, Halsey and Henderson were tested to the equilibrium data. Kinetic studies based on Lagergren first-order, pseudo-second-order rate expressions and intra-particle diffusion studies were done. The batch experiments were conducted at room temperature (30ºC) and at the normal pH (6.7) of the solution. It was observed that Hg(II) removal rate was better for FE than AC, and the adsorption capacity of AC (69.44 mg/g) was found to be much better than FE (1.15 mg/g). Hybrid fractional error function analysis showed that the best-fit for the adsorption equilibrium data were represented by Freundlich isotherm. Kinetic and filmdiffusion studies showed that the adsorption of mercury on FE and AC was both intra-particle diffusion and film-diffusion controlled. In a study by Abu-El-Sha‟r and Haddad (2007), lead adsorption onto soil samples from Irbid, which were subjected to high temperatures, was investigated. These samples were collected from ground surface and heated to temperatures of 25, 70, 100, 200, 225, 250, 275, 300, 400, and 550°C. Based on these temperatures the soil was divided into ten different groups. Each group was first characterized by conducting a set of experiments to estimate the liquid limit (LL), plastic limit (PL), and plasticity index, the organic carbon content, and a set of batch experiments to study lead adsorption. Results indicated that the LL, PL, total organic carbon were slightly affected by high temperatures less than 200°C, showed an abrupt change between temperature from 200 and 300°C, and then slight change above 300°C. Adsorption of lead onto heated samples, however, was not significantly changed. This may be explained by the fact that adsorption of heavy metals mainly occurs onto the soil mineral parts which are slightly affected by the temperature range used in this study. The adsorption of Pb(II) onto Turkish (Bandirma region) kaolinite clay was examined in aqueous solution with respect to the pH, adsorbent dosage, contact time, and temperature by Sari et al. (2007). The linear Langmuir and Freundlich models were applied to describe equilibrium isotherms and both models fitted well. The monolayer adsorption capacity was found as 31.75 mg/g at pH 5 and 20 °C. Dubinin–Radushkevich isotherm model was also applied to the equilibrium data. The mean free energy of adsorption (13.78 kJ/mol) indicated that the adsorption of Pb(II) onto kaolinite clay may be carried out via chemical ion-exchange mechanism. The adsorption of Pb(II) onto kaolinite clay was feasible, spontaneous and exothermic in nature. Furthermore, the experimental data fitted well with the pseudo-secondorder kinetics. Removal of copper and zinc from aqueous solutions was investigated by Veli and Alyüz, (2007) using Cankiri bentonite natural clay. The effects of pH, clay amount, heavy metal
Carbons and Clays for Heavy Metals Removal …
29
concentration and agitation time on adsorption efficiency were studied. Langmuir, Freundlich and Dubinin–Radushkevich isotherms were applied in order to determine the efficiency of natural clay used as an adsorbent. Results showed that all isotherms were linear. It was observed that adsorption data of Cu(II) and Zn(II) were well-fitted by the second-order reaction kinetics. In addition, calculated and experimental heavy metal amounts adsorbed by the unit clay mass were too close to each other. It was concluded that natural clay could be used as an effective adsorbent for removing Cu(II) and Zn(II) from aqueous solutions. A work by Santos and Masini (2007) presented an evaluation of vermiculite as a low cost adsorbent for treatment of wastewater from a coatings industry containing Cd(II), Pb(II) and Cu(II). Adsorption data were fitted by Freundlich isotherms, as well as by partition constants at pH 4, 5 and 6. It was observed that the non-expanded vermiculite presented the following affinity orders by the studied ions: pH 4: Cu(II) < Cd(II) < Pb(II); pH 5: Cu(II) ≈ Cd(II) < Pb(II); pH 6: Cd(II) < Cu(II) < Pb(II). For Pb(II) and Cd(II), the adsorption percentages determined in real wastewaters were around 20% lower than the removal percentage previewed by the Freundlich parameters, a fact that may be explained by competition of the studied cations among themselves, and with Fe(III) species, which were present in the water at concentration levels similar to Cd(II), Cu(II) and Pb(II). Additionally, the high content of organic compounds in the wastewater might have decreased the adsorption of Cu(II) and Pb(II) because of possible formation of soluble complexes between the heavy metal cations and the organic compounds. On the other hand, adsorption of Cd(II) from the real wastewater was about 20% higher than that previewed by the Freundlich parameters, denoting the complexity of interactions that ions are liable in matrices of wastewaters. A series of activated palygorskite clays by HCl with different concentrations were prepared and applied as adsorbents for removal of Cu(II) from aqueous solutions by Chen et al. (2007). The results showed that adsorption capacity of activated palygorskites increased with increasing the HCl concentration and the maximum adsorption capacity with 32.24 mg/g for Cu(II) was obtained at 12 mol/L of HCl concentration. Kinetic studies indicated that the adsorption mechanisms in the Cu(II)/acid-activated palygorskite system followed the pseudosecond-order kinetic model with a relatively small contribution of film-diffusion. Equilibrium data fitted well with the Freundlich isotherm model compared to the Langmuir isotherm model, indicating that adsorption taking place on heterogeneous surfaces of the acid-activated palygorskite. The use of natural palygorskite clay for the removal of Pb(II) from aqueous solutions for different contact times, pH of suspension, adsorbent amounts and particle sizes of palygorskite clay were investigated by Chen and Wang (2007). Batch adsorption kinetic experiments revealed that the adsorption of Pb(II) onto palygorskite clay involved fast and slow processes. It was found that the adsorption mechanisms in the lead/palygorskite system followed pseudo-second-order kinetics with a significant contribution from film-diffusion. The Langmuir model represented the adsorption process better than the Freundlich model. The maximum adsorption capacity of Pb(II) onto natural palygorskite was found to be 104.28 mg/g. Adsorption of Pb(II) ions from aqueous solution onto clinoptilolite was investigated by Günay et al. (2007) to evaluate the effects of contact time, initial concentration and pretreatment of clinoptilolite on the removal of Pb(II). Maximum experimental adsorption capacity was found to be 80.933 and 122.400 mg/g for raw and pretreated clinoptilolite,
30
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
respectively, for the initial concentration of 400 mg/L. Results of the kinetic studies showed that the best fitted kinetic models were obtained to be in the order: the pseudo-first-order, the pseudo-second-order and Elovich equations. The negative value of change in Gibbs free energy (ΔG°) indicates that the adsorption of Pb(II) on clinoptilolite was spontaneous. Bhattacharyya and Gupta (2007) investigated the influence of acid activation of montmorillonite on adsorption of Cd(II), Co(II), Cu(II), Ni(II), and Pb(II) from aqueous medium and comparison of the adsorption capacities with those on parent montmorillonite. The clay-metal interactions were studied under different conditions of pH, concentration of metal ions, amount of clay, interaction time, and temperature. The interactions were dependent on pH and the uptake was controlled by the amount of clay and the initial concentration of the metal ions. The adsorption capacity of acid-activated montmorillonite increased for all the metal ions. The interactions were adsorptive in nature and relatively fast and the rate processes were more akin to the second-order kinetics. The Langmuir monolayer capacity of the acid-activated montmorillonite was more than that of the parent montmorillonite (Cd(II): 32.7 and 33.2 mg/g; Co(II): 28.6 and 29.7 mg/g; Cu(II): 31.8 and 32.3 mg/g; Pb(II): 33.0 and 34.0 mg/g; and Ni(II): 28.4 and 29.5 mg/g for montmorillonite and acid-activated montmorillonite, respectively). The thermodynamics of the rate processes showed that the adsorption of Co(II), Pb(II), and Ni(II) to be exothermic, accompanied by decreases in entropy and Gibbs free energy, while the adsorption of Cd(II) and Cu(II) was endothermic, with an increase in entropy and an appreciable decrease in Gibbs free energy. The results established the potential use of montmorillonite and its acid-activated form as adsorbents for Cd(II), Co(II), Cu(II), Ni(II), and Pb(II) ions from aqueous media. Application of riverbed sand for the adsorptive separation of Cd(II) from aqueous solutions has been investigated by Sharma et al. (2007). Metal removal increased from 26.8 to 56.4% by decreasing the initial concentration of cadmium from 7.5 × 10−5 to 1.0 × 10−5 M at pH 6.5, 25 °C temperature, agitation speed of 100 rpm, 100 μm particle size and 1.0 × 10−2 NaClO4 ionic strength. Process of separation is governed by first-order rate kinetics. Values of thermodynamic parameters ΔGo, ΔHo and ΔSo were also calculated and were recorded as −0.81 kcal/mol, −9.31 kcal/mol and −28.10 kcal/mol, respectively, at 25°C. The solution pH has been found to affect the removal of cadmium significantly and maximum removal (58.4%) has been found at pH 8.5. In a work by Shawabkeh et al. (2007), natural bentonite was treated by hydrochloric, nitric, and phosphoric acids followed by washing with sodium hydroxide in order to enhance its adsorption capacity. The sample which was treated with hydrochloric acid, followed by further treatment with NaOH, showed the highest cation exchange capacity with a value of 51.20 meq/100 g. Adsorption isotherms for both cobalt and zinc were fitted using Langmuir, Freundlich, and Redlich-Peterson and showed an adsorption capacity of 138.1 mg Co(II) and 202.6 mg Zn(II) per gram of treated adsorbent sample. The adsorption characteristics of palygorskite with respect to cadmium were studied with the aim of assessing its use in water purification systems by Álvarez-Ayuso and GarcíaSánchez (2007). The adsorption of Cd on palygorskite appeared as a fast process, with equilibrium being attained within the first half-an-hour of interaction. This process was described by the Langmuir model and gave a maximum Cd sorption of 4.54 mg/g. This sorption capacity value was greatly affected by both pH and ionic strength. High competing electrolyte concentrations have decreased the amount of Cd sorbed (close to 60%), suggesting a great contribution of replacement of exchange cations in this metal removal by palygorskite.
Carbons and Clays for Heavy Metals Removal …
31
The increase of mineral dose provoked a Cd removal raise; removal values in the range of 8545% were attained for Cd initial concentrations of 10–150 mg/L (0.089–1.34 mmol/L) when the palygorskite dose of 20 g/L was employed. Column studies were also performed in order to estimate the potential of palygorskite to be used in continuous flow purification systems, showing the effectiveness of this mineral to purify, down to the legal limit of waste, moderate volumes of Cd-containing solutions with a similar concentration (50 mg/L or 0.445 mmol/L) to those mostly found in the upper range of concentrations usually present in industrial wastewaters. In a study by Kubilay et al. (2007), the removal of Cu(II), Zn(II) and Co(II) ions from aqueous solutions using adsorption onto natural bentonite was investigated as a function of initial metal concentration, pH and temperature. For all the metal cations studied, the maximum adsorption was observed at 20°C. The batch method was employed using initial metal concentrations ranging from 15 to 70 mg/L at pH 3.0, 5.0, 7.0 and 9.0. It was found that in every concentration range, adsorption data of bentonitic clay - heavy metal cations, matched to Langmuir, Freundlich and Dubinin-Kaganer-Radushkevich (DKR) isotherms. Bentonite used was sensitive to pH changes and the amounts of heavy metal cations adsorbed increased as pH was increased in adsorbent-adsorbate system. According to the adsorption equilibrium studies, the selectivity order was found to be: Zn(II)>Cu(II)>Co(II). These results showed that bentonitic clay holds great potential to remove the relevant heavy metal cations from wastewater. The sorption of Cr(III) from aqueous solutions on kaolinite was studied by a batch technique by Turan et al. (2007). The adsorbed amount of chromium ions on kaolinite increased with increasing pH and temperature and decreased with increasing ionic strength. The sorption of Cr(III) on kaolinite was found to be endothermic. Sorption data have been interpreted in terms of Freundlich and Langmuir equations. The experimental data were correlated reasonably well by the Langmuir adsorption isotherm. The enthalpy change for chromium adsorption was estimated to be 7.0 kJ/mol. In a work by Manohar et al. (2006), a natural bentonite clay collected from Ashapura Clay Mines, Gujarat State, India, was utilized as a precursor to produce aluminum-pillared bentonite clay (Al-PILC) for the removal of Co(II) ions from aqueous solutions. Adsorption experiments were conducted under various conditions, i.e., pH, contact time, initial concentration, ionic strength, adsorbent dose and temperature. The most effective pH range for the removal of Co(II) ions was found to be 6.0–8.0. The maximum adsorption of 99.8% and 87.0% took place at pH 6.0 from an initial concentration of 10.0 and 25.0 mg/L, respectively. Kinetic studies showed that an equilibrium time of 24 h was needed for the adsorption of Co(II) ions on Al-PILC and the experimental data were correlated by the external mass transfer diffusion model for the first-stage of adsorption and the intraparticle mass transfer diffusion model for the second-stage of adsorption. The intraparticle mass transfer diffusion model gave a better fit to the experimental data. The equilibrium isotherm data were analyzed using the Langmuir, Freundlich and Scatchard isotherm equations and the adsorption process was expressed by Freundlich isotherm. The adsorption behavior of vermiculite was studied with respect to cadmium, copper, lead, manganese, nickel, and zinc as a function of pH and in the presence of different ligands by Malandrino et al. (2006). The continuous column method was used in order to evaluate the feasibility to use the clay in wastewater purification systems. The total capacity of vermiculite was found to increase in the following order: Mn > Ni > Zn > Cd > Cu > Pb. The adsorption
32
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
of metal ions on vermiculite decreased with decreasing pH and increasing ionic strength. The metal uptake on the clay was hindered by the presence of strong complexing agents in solution and it decreased with increasing of the complexation of the ligands with exception of cysteine and tiron. It was concluded that the vermiculite has good potentialities for costeffective treatments of metal-contaminated wastewaters. Natural Jordanian adsorbent (consisting of quartz and aluminosilicates and secondary minerals, i.e., calcite and dolomite) was shown to be effective for removing Zn(II), Pb(II) and Co(II) from aqueous solution as reported by Al-Degs et al. (2006). The major mineral constituents of the sorbent were calcite and quartz. Dolomite was present as minor mineral and palygorskite was present as trace mineral. The sorbent had microporous structure with a modest surface area of 14.4 m2/g. The adsorption capacities of the metals were: 2.86, 0.32, 0.076 mmol cation/g for Zn(II), Pb(II) and Co(II) at pH 6.5, 4.5 and 7.0, respectively. Adsorption data of metals were described by Langmuir and Freundlich models over the entire concentration range. It was found that the mechanism of metal adsorption was mainly due to the precipitation of metal carbonate complexes. The overall adsorption capacity has decreased after acid treatment, as this decreases the extent of precipitation on calcite and dolomite. Kinetic data were accurately fitted to pseudo-first-order and external diffusion models, which indicated that adsorption of Zn(II) occurred on the exterior surface of the adsorbent and the contribution of internal diffusion mechanism was insignificant. Gupta and Bhattacharyya (2006) investigated the adsorptive interactions of Ni(II) ions with kaolinite, montmorillonite, and their poly(oxo-zirconium) and tetrabutylammonium (TBM) derivatives in aqueous medium. The adsorption strongly depended on pH of the medium with enhanced adsorption as the pH turns from acidic to alkaline side till precipitation started. The process was fast initially and maximum adsorption was observed within 180 min of agitation. The kinetics of the interactions showed better agreement with second-order kinetics. The adsorption data gave Langmuir monolayer capacity of 2.75 to 21.14 mg/g for the clay adsorbents. The adsorption process was exothermic accompanied by decrease in entropy and Gibbs free energy. The results showed that montmorillonite had the largest adsorption capacity followed by ZrO-montmorillonite, TBA-montmorillonite, kaolinite, ZrO-kaolinite and TBA-kaolinite. Introduction of ZrO- and TBA- groups into the clays reduced their adsorption capacity by blocking the available adsorption sites. Bhattacharyya and Gupta (2006) investigated the removal of Fe(III) ions from an aqueous solution using kaolinite, montmorillonite and their acid activated forms. The specific surface areas of kaolinite, acid activated kaolinite, montmorillonite and acid activated montmorillonite were 3.8, 15.6, 19.8 and 52.3 m2/g, respectively, whereas the cation exchange capacity (CEC) was measured as 11.3, 12.2, 153.0, and 341.0 meq/100g for the four clay adsorbents, respectively. Adsorption increased with pH till Fe(III) became insoluble at pH > 4.0. The second-order kinetics (k2 = 4.7×10− 2 to 7.4×10− 2 g/mg/min) gave a better description of the kinetic data. The Langmuir monolayer capacity of the clay adsorbents was from 11.2 to 30.0 mg/g. The adsorption was exothermic with ΔHo in the range of −27.6 to −42.2 kJ/mol accompanied by decrease in entropy (ΔSo = −86.6 to −131.8 J/mol/K) and decrease in Gibbs free energy. The results showed that the kaolinite, montmorillonite and their acid activated forms could be used as adsorbents for separation of Fe(III) from aqueous solution. Acid activation enhanced the adsorption capacity as compared to the untreated clay minerals.
Carbons and Clays for Heavy Metals Removal …
33
A study was carried out by Sprynskyy et al. (2006) on the adsorption of heavy metals (Ni(II), Cu(II), Pb(II), and Cd(II)) from single- and multi-component aqueous solutions by raw and pretreated clinoptilolite. The adsorption had ion-exchange nature and consisted of three stages, i.e., the adsorption on the surface of microcrystals, the inversion stage, and the moderate adsorption in the interior of the microcrystals. The finer clinoptilolite fractions adsorbed higher amounts of the metals due to relative enrichment by the zeolite proper and higher cleavage. The slight difference between adsorption capacity of the clinoptilolite toward lead, copper, and cadmium from single- and multi-component solutions testified to individual adsorption centers of the zeolite for each metal. The decrease of nickel adsorption from multicomponent solutions was probably caused by the closeness of its adsorption forms to the other metals and by competition. The maximum sorption capacity towards Cd(II) was determined as 4.22 mg/g at an initial concentration of 80 mg/L and towards Pb(II), Cu(II), and Ni(II) as 27.7, 25.76, and 13.03 mg/g, respectively, at 800 mg/L of initial concentration. The adsorption results fitted well to the Langmuir model. Vermiculite, a 2:1 clay mineral, was applied as adsorbent for removal of cadmium, zinc, manganese, and chromium from aqueous solutions by Fonseca et al. (2006). All isotherms observed were L-type of the Gilles classification, except zinc (S-type). The adsorbent showed good adsorption potential for these cations. The experimental data were analyzed by the Langmuir isotherm model showing reasonable adjustment. The quantity of adsorbed cations was 0.50, 0.52, 0.60, and 0.48 mmol/ g of Cd(II), Mn(II), Zn(II), and Cr(II), respectively. Manohar et al. (2005) investigated the possibility of using a natural bentonite clay as a precursor to produce aluminum-pillared clay (Al-PILC) for the removal of vanadium(IV) from aqueous solutions. Batch experiments were carried out as a function of solution pH, contact time, vanadium(IV) concentration, adsorbent dose, ionic strength, and temperature. The maximum adsorption capacity was observed in the pH range of 4.5−6.0. The maximum adsorption of 99.8 and 88.5% took place at pH 5.0 from an initial concentration of 5 and 10 mg/L, respectively. It was shown that the adsorption of vanadium(IV) could be fitted to the intra-particle mass-transfer model. The temperature dependence indicated the endothermic nature of adsorption. The percentage removal of vanadium(IV) decreased with increasing ionic strength. The Freundlich isotherm was found to well represent the measured adsorption data. Kaolin (bright white lumps) from Ubulu-Ukwu in Nigeria was modified with 200 μg/mL of phosphate and sulphate anions to give phosphate- and sulfate-modified adsorbents, respectively and the adsorption of four metal ions (Pb(II), Cd(II), Zn(II), and Cu(II)) was studied as a function of metal ions concentration by Adebowale et al. (2005). The metal ions showed stronger affinity for the phosphate-modified adsorbent with Pb(II), Cu(II), Zn(II), and Cd(II) giving an average of 93.28%, 80.94%, 68.99%, and 61.44% uptake capacity, respectively. The order of preference for the various adsorbents shown by the metal ions was as follows: Pb(II) > Cu(II) > Zn(II) > Cd(II). Desorption studies showed that the phosphatemodified adsorbent had the highest affinity for the metal ions, followed by the sulfatemodified clay, while the unmodified clay had the least affinity. The experimental data were fitted by both the Langmuir and Freundlich models. In a study, Srivastava et al. (2005) investigated the adsorption of Cd(II), Cu(II), Pb(II), and Zn(II) onto kaolinite in single- and multi-element systems as a function of pH and concentration, in a background solution of 0.01 M NaNO3. The pH was varied from 3.5 to 10.0 with total metal concentration of 133.3 μM in the single-element system and 33.3 μM
34
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
each of Cd(II), Cu(II), Pb(II), and Zn(II) in the multi-element system. The value of pH50 (the pH at which 50% adsorption occurs) was found to follow the sequence Cu < Zn < Pb < Cd in single-element systems, but Pb < Cu < Zn < Cd in the multi-element system. Adsorption isotherms at pH 6.0 in the multi-element systems showed that there was competition among various metals for adsorption sites on kaolinite. The adsorption and potentiometric titrations data for various kaolinite-metal systems were modeled using an extended constantcapacitance surface complexation model that assumed an ion-exchange process below pH 7.0 and the formation of inner-sphere surface complexes at higher pH. Inner-sphere complexation was more dominant for the Cu(II) and Pb(II) systems. The adsorption of the heavy metals (Cd(II), Cu(II), Mn(II), Pb(II), and Zn(II)) from aqueous solutions by a natural Moroccan stevensite was studied by Benhammou et al. (2005a). The surface area of stevensite was 134 m2/g and the cation exchange capacity (CEC) was 76.5 meq/100 g. Adsorption tests of Cd(II), Cu(II), Mn(II), Pb(II), and Zn(II) in batch reactors were carried out at ambient temperature and at constant pH. The increasing order of the adsorption rates followed the sequence: Mn(II) > Pb(II) > Zn(II) > Cu(II) > Cd(II). The maximal adsorption capacities at pH 4.0 determined from the D–R and Langmuir models vary in the following order: Cu(II) > Mn(II) > Cd(II) > Zn(II) > Pb(II). The equilibrium data fitted well with the three-parameter Redlich–Peterson model. The values of mean energy of adsorption show mainly an ion-exchange mechanism. The objective of a study by Benhammou et al. (2005b) was to investigate the adsorption of the heavy metals Hg(II) and Cr(VI), from aqueous solutions, onto Moroccan stevensite. In order to improve the adsorption capacity of stevensite for Cr(VI), a preparation of stevensite was carried out. It consisted of saturating the stevensite in ferrous iron Fe(II) and reducing the total Fe by Na2S2O4. Then, the adsorption experiments were studied in batch reactors at 25 °C. The influence of the pH solution on the Cr(VI) and Hg(II) adsorption was studied in the pH range of 1.5-7.0. The optimum pH for the Cr(VI) adsorption was in the pH range of 2.0-5.0, and for Hg(II) above 4.0. The adsorption kinetics was tested by a pseudo-secondorder model. The adsorption rate of Hg(II) was 54.35 mmol/kg-min and that of Cr(VI) was 7.21 mmol/kg-min. The adsorption isotherms were described by the Dubinin-Radushkevich model. The maximal adsorption capacity for Cr(VI) increased from 13.7 (raw stevensite) to 48.86 mmol/kg (modified stevensite) and for Hg(II) it decreased from 205.8 to 166.9 mmol/kg. A study was carried out by Sarioglu et al. (2005) to examine the removal of copper from an aqueous solution by phosphate rock (PR). The optimum conditions for adsorption were evaluated by changing various parameters, viz., effects of pH, adsorbent concentration, initial metal concentration and contact time. The study showed that copper removal from an aqueous solution increased with increasing pH and adsorbent concentration (up to 5 g/L) and decreased with increasing initial copper concentration, and the equilibrium (contact) time was 40 min. The adsorption capacity of PR was determined as 0.17 mmol/g by fitting the experimental results to Langmuir isotherm. The potential of using activated phosphate as a new adsorbent for the removal of Pb from aqueous solutions was investigated by Mouflih et al. (2005). The kinetics of lead adsorption and the adsorption process were compared for natural phosphate (NP) and activated phosphate (AP). The results indicate that equilibrium was established in about 1 h for NP and 3 h for AP. The effect of the pH was examined in the range of 2–6 and the maximum removal obtained was between 2 and 3 for NP and between 3 and 4 for AP. The maximum adsorption
Carbons and Clays for Heavy Metals Removal …
35
capacities at 25 °C were 155.04 and 115.34 mg/g for AP and NP, respectively. The thermodynamic parameter showed that adsorption of lead on NP and AP was an endothermic process. These results showed that AP was a good adsorbent for heavy metals from aqueous solutions and could be used as a purifier for water and wastewater. Kinetic and equilibrium adsorption experiments on removal of Zn(II) from aqueous solutions by scoria (a vesicular pyroclastic rock with basaltic composition) from Jeju Island, Korea, in order to examine its potential use as an efficient sorbent, was conducted by Kwon et al. (2005). The batch-type kinetic sorption tests under variable conditions indicated that the percentage of Zn(II) removal by scoria increased with decreasing initial Zn(II) concentration, particle size, and sorbate/sorbent ratio. However, the adsorption capacity decreased with the decrease of initial Zn(II) concentration and sorbate/sorbent ratio. Equilibrium adsorption tests showed that Jeju scoria had a larger capacity and affinity for Zn(II) sorption than commercial powdered activated carbon (PAC), at initial Zn(II) concentrations of more than 10 mM, the adsorption capacity of Jeju scoria was about 1.5 times higher than that of PAC. The acquired adsorption data better fitted to the Langmuir isotherm. The adsorption behavior was mainly controlled by cation exchange and typically displayed characteristics of „cation sorption‟. The Zn(II) removal capacity decreased when solution pH decreased because of the competition with hydrogen ions for adsorption sites, while the Zn(II) removal capacity increased under higher pH conditions, which was likely due to hydroxide precipitation. At an initial Zn(II) concentration of 5.0 mM, the removal increased from 70% to 96% with the increase of initial pH from 3.0 to 7.0. The kinetics of sorption of Cu(II) on a Saudi clay mineral (bentonite) was investigated by Al-Qunaibit et al. (2005) at 20ºC using different weights of the clay (0.5, 1.0, 1.5, and 2 g). Each weight represented a certain sample size. The order of the process appeared to be 1 with respect to Cu(II), and 1½ with respect to the clay surface area. The adsorption rate was found to depend on internal diffusion, which produced certain decrease in the specific rate of sorption as a function of time. Adsorption characteristics were described using two-site Langmuir isotherm. The desorption experiments proved that Cu(II) ions were chemisorbed on the bentonite surface. The maximum adsorption obtained was 909 mg Cu(II)/g clay. Calcined phosphate (CP) was evaluated as a new adsorbent for removal of heavy metals from aqueous solution by Aklil et al. (2004). Removal of Pb(II), Cu(II), and Zn(II) on the CP was investigated in batch experiments. The influence of pH was studied and the adsorption capacities obtained at pH 5 were 85.6, 29.8, and 20.6 mg/g for Pb(II), Cu(II) and Zn(II), respectively. The adsorption between phosphate rock (PR) and metals (Pb, Cu, and Zn) was studied by Cao et al. (2004). Phosphate rock had the highest affinity for Pb, followed by Cu and Zn, with sorption capacities of 138, 114, and 83.2 mmol/kg PR, respectively. In the Pb–Cu–Zn ternary system, competitive metal sorption occurred with adsorption capacity reduction of 15.2%, 48.3%, and 75.6% for Pb, Cu, and Zn, respectively, compared to the mono-metal systems. A fractional factorial design showed the interfering effects in the order of Pb > Cu > Zn. The capacity of sepiolite for the removal of lead ions from aqueous solution was investigated under different experimental conditions by Bektaş et al. (2004). The Langmuir and Freundlich equations were applied to fit the data. The constants and correlation coefficients of these isotherm models at different conditions, such as pH, temperature and particle size were calculated and compared. The equilibrium process was well described by the Langmuir isotherm model and the maximum sorption capacity was found to be 93.4 mg/g
36
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
for the optimal experimental conditions. The best correlation coefficients were obtained using the pseudo-second-order kinetic model. Removal of heavy metals Mn(II), Co(II), Ni(II), and Cu(II) from aqueous solutions was studied using a raw kaolinite by Yavuz et al. (2003). The adsorption of these metals on kaolinite conformed to linear form of Langmuir adsorption equation. Langmuir adsorption capacity for each metal was found as 0.446 mg/g (Mn), 0.919 mg/g (Co), 1.669 mg/g (Ni), 10.787 mg/g (Cu) at 25°C. The thermodynamic parameters showed that the adsorption of these heavy metals on kaolinite were an endothermic process. Dho and Lee (2003) conducted a combined adsorption-sequential extraction analysis by which five phases (i.e., exchangeable, carbonate, Mn-Oxide, organic, and Fe-Oxide phases) of adsorbed heavy metals were analyzed, to investigate temperature effects on single and competitive adsorptions of Zn(II) and Cu(II) onto natural clays. In the case of single adsorption of Zn, the exchangeable phase adsorption decreased from 65 to 40%, but the carbonate phase adsorption increased from 30 to 40%, with an increase in temperature from 15 to 55°C. However, in its competitive adsorption with Cu, Zn was mostly present in the exchangeable phase (over 90%), and with an increase in temperature, the exchangeable phase adsorption decreased only 10%. In the case of Cu, over 50% among the total amount of adsorption was present in the carbonate phase in both cases of single and competitive adsorptions. The carbonate phase adsorption of Cu increased from 56 to 61% and from 60 to 66% in single and competitive adsorptions, respectively, with a temperature increase. These results showed that in the case of Zn, the major mechanism of retention in natural clay soils could be exchangeable phase adsorption, especially in the case of competitive adsorption with Cu. However, in the case of Cu, the major mechanism could be carbonate phase adsorption. It was observed that the adsorption of Zn and Cu onto natural clays was endothermic, which indicated that the adsorption equilibrium constants and capacities increase with a temperature increase, with the exception of exchangeable phase adsorption. The adsorption behavior of sepiolite was studied with respect to cadmium and zinc in order to consider its application to remediate soils polluted with these metals by ÁlvarezAyuso and García-Sánchez (2003a). The Langmuir model was found to describe the sorption processes well, offering maximum sorption capacities of 17.1 and 8.13 mg/g for cadmium and zinc, respectively, at pH 6. The sorption capacities were pH dependent, undergoing a decrease with H+ concentration increase. The column studies also showed a high reduction in the leaching of cadmium and zinc (69 and 52%, respectively) when a sepiolite dose of 4% was applied. The adsorption behavior of palygorskite was studied with respect to lead, copper, zinc and cadmium in order to consider its application to remediate soils polluted with these metals by Álvarez-Ayuso and García-Sánchez (2003b). The Langmuir model was found to describe the adsorption processes well offering maximum sorption values of 37.2 mg/g for lead, 17.4 mg/g for copper, 7.11 mg/g for zinc and 5.83 mg/g for cadmium at pH 5–6. The column studies also showed a high reduction in the metal leaching (50% for lead, 59% for copper, 52% for zinc and 66% for cadmium) when a palygorskite dose of 4% was applied. The adsorption characteristics of heavy metals such as Cd(II), Cr(III), Cu(II), Ni(II), Pb(II), and Zn(II) ions by kaolin (kaolinite) and ballclay (illite) from Thailand were studied by Chantawong et al. (2003). It was found that, except Ni, metal adsorption increased with increased pH of the solutions and their adsorption followed both Langmuir and Freundlich isotherms. Adsorption of metals in the mixture solutions by kaolin was: Cr > Zn > Cu ≈ Cd ≈
Carbons and Clays for Heavy Metals Removal …
37
Ni > Pb, and for ballclay was: Cr > Zn > Cu > Cd ≈ Pb > Ni. The adsorption of metals was endothermic, with the exception of Cd, Pb and Zn for kaolin, Cu and Zn for ballclay. The presence of Cr(III) induced the greatest reduction of metal adsorption onto kaolin, as did the presence of Cu(II) for ballclay. A bentonite and an expanded perlite (Morocco) were used for the removal of trivalent chromium from aqueous solutions by Chakir et al. (2002). The kinetic study showed that the uptake of Cr(III) by bentonite was very rapid as compared to expanded perlite. For both the adsorbents the adsorption capacity increased with increasing pH of the suspensions. Results showed that bentonite was more effective in removing trivalent chromium (96%) from aqueous solution than expanded perlite (40%). Surface complexation played an important role in the sorption of Cr(III) species on expanded perlite. In the case of bentonite, cationexchange was the predominate mechanism for adsorption of trivalent chromium ions. A thiol-functionalized layered magnesium phyllosilicate material (Mg-MTMS) was investigated as a high-capacity adsorbent for heavy metal ions by Lagadic et al. (2001). Structural characterization by powder X-ray diffraction, infrared spectroscopy, NMR spectroscopy and elemental analyses confirmed the smectite-type structure. Mg-MTMS was found to be highly effective for the adsorption of Hg(II), Pb(II), and Cd(II) ions, exhibiting extraordinary metal ion uptake capacities of 603, 365, and 210 mg of metal/g of adsorbent, respectively. The high effectiveness of Mg-MTMS for the capture of metal ions is attributed to both high concentration of complexing thiol groups (6.4 mmol of SH/g of Mg-MTMS) and expansion capability of the framework, which facilitates the accessibility of the binding sites. De-oiled spent bleaching clay was activated either by acid treatment followed by heat activation or by heat activation alone at temperatures between 200 and 800°C by Seng et al. (2001). The surface area of the heat-activated clay attained a maximal value of ≈120 m2/g at temperatures between 400 and 500°C, while the acid-heat-treated clay attained maximal surface area of ≈140 m2/g. The adsorption capacities of Cr(VI) for both series studied increased as the activation temperature increased until 300°C and decreased again at higher temperatures. At lower pH, more than 95% of the Cr(VI) was absorbed in a solution with initial concentration of 1 mg/L per gram of adsorbent activated at 300°C. The adsorption patterns followed Freudlich isotherm. The amount of Ni(II) adsorbed increased with the pH of the solution for all samples studied. The maximal adsorption capacities of the adsorbents in solution containing initial Ni(II) concentration of 5 mg/L per 0.5 g of adsorbent and at pH 6 were found to be 44 and 42%, respectively, for the acid-treated sample activated at 500°C and for the nonacid-treated sample activated at 700°C. The use of an adsorbent produced by the chemical treatment of locally available clay for the removal of some metals from waste water was investigated by Vengris et al. (2001). The modification of the natural clay was performed by treatment with hydrochloric acid and subsequent neutralization of the resultant solution by sodium hydroxide. The adsorption amounts of iron, aluminium and magnesium compounds were increased with the modified sorbent. Acidic treatment led to the decomposition of the montmorillonite structure. Adsorption studies were carried out by both batch and column methods. The uptake capacity of the modified clay for nickel, copper and zinc significantly increased. Batch and column sorption methods enabled the removal of nickel, copper and zinc ions till the permissible sewerage discharge concentration. The sorption process was reflected by Langmuir-type isotherm.
38
John U. Kennedy Oubagaranadin and Z.V.P. Murthy Table 3.2. Clay adsorbents for heavy metals from solutions Type of clay
Adsorbate metal ion Ni(II)
Calcined Bofe bentonite clay Smectite with a small Cr(III) proportion of kaolinite (From Jebel Chakir, Tunisia, North Africa). Tabuk and Khaiber (From Pb(II) Saudi Arabia) Kaolin Pb(II) Petra clay Cd(II), Pb(II) Montmorillonite – Illite clay Pb(II) White, yellow and red sands Cr(III) from the United Arab Emirates Raw and acid-activated Cu(II) bentonite Modified Unye bentonite Cu(II) Tunisian smectite-rich clay Pb(II) Spent activated clay Cr(VI) Kaolinite and Fe(III), Co(II), montmorillonite Ni(II) Bentonite Pb(II) Natural clinoptilolite Zn(II) Diatomite Cr(III) Laboratory grade Fuller‟s Hg(II) earth Turkish kaolinite Pb(II) Activated palygorskite Cu(II) Natural palygorskite Pb(II) Clinoptilolite Pb(II) Montmorillonite Cd(II), Co(II), Cu(II), Ni(II), Pb(II) Palygorskite Cd(II) Natural and activated phosphate Saudi bentonite Calcined phosphate Sepiolite Raw kaolinite Sepiolite Palygorskite
Adsorption capacity, Reference qm (mg/g) 1.91 Vieira et al., 2010 117.5
Ghorbel-Abid et al., 2009
30, 10 4.2 74.07, 83.33 Raw: 52 Acid activated: 78 62.5, 9.8, 2.38
Al-Jlil and Alsewailem, 2009 Jiang et al., 2009 Baker, 2009 Oubagaranadin and Murthy, 2009c and 2010 Khamis et al., 2009
42.41, 32.17
Eren and Afsin, 2008
105.38 25 1.422 10.4 to 11.2 28.4 to 28.9 78.82 21.2 26.5 1.15
Eren, 2008 Chaari et al., 2008 Weng et al., 2008 Bhattacharyya and Gupta, 2008 Zhu et al., 2008 Çoruh, 2008 Gürü et al., 2008 Oubagaranadin et al., 2007
31.75 32.24 104.28 80.93 32.7, 28.6, 31.8, 28.4, 33.0
Sari et al., 2007 Chen et al., 2007 Chen and Wang, 2007 Günay et al., 2007 Bhattacharyya and Gupta, 2007
4.54
Pb(II)
115.34, 155.04
Álvarez-Ayuso and GarcíaSánchez, 2007 Mouflih et al., 2005
Cu(II) Pb(II), Cu(II), Zn(II) Pb(II) Mn(II), Co(II), Ni(II), Cu(II) Cd(II), Zn(II)
909 85.6, 29.8, 20.6
Al-Qunaibit et al., 2005 Aklil et al., 2004
93.4 0.446, 0.919, 1.669, 10.787 17.1, 8.13
Bektaş et al., 2004 Yavuz et al., 2003
Pb(II), Cu(II), Zn(II), Cd(II)
Álvarez-Ayuso and GarcíaSánchez, 2003ª 37.2, 17.4, 7.11, 5.83Álvarez-Ayuso and GarcíaSánchez, 2003b
Rashed (2001) reported suitable conditions for the use of naturally occurring minerals (talc, chalcopyrite and barite) as adsorbents for the removal of lead ions. The adsorption of lead ions from solutions containing different initial lead concentrations (50, 100, 200, 400, 600, 800 and 1000 mg/L Pb as lead nitrate) using different size fractions (<63μm, 63–150μm) of talc, chalcopyrite and barite at different pH (3, 5, 7 and 9) and different adsorption times (24, 48, 72 and 96 h) was examined. The results revealed that the chalcopyrite fraction
Carbons and Clays for Heavy Metals Removal …
39
between 63–150μm showed the highest adsorption capacity. It was concluded that the equilibrium time of adsorption was 72 h at optimum pH between 7–9. Amorphous derivatives of kaolinites prepared by thermal modification followed by acid activation which improved the exchangeability of kaolinites were studied by Suraj et al. (1998). Adsorption of cadmium and copper on these modified kaolinites was studied as a function of equilibration time and temperature and it was found that the initial 1 h was sufficient to exchange most of the metal ions. Two kaolinitic clay samples obtained from Thonnakkal, south Kerala (TK) and Madai, north Kerala (MK) were modified to study their exchange behaviour. The exchangeability was found to decrease with an increase in the calcination temperature (to 600°C) of kaolinite samples. An improved exchange kinetics applies for their modified (calcined and acid activated) counterparts. The amount of metal ions adsorbed showed a direct correlation with the surface area and cation exchange capacity (CEC) values. The uptake of Cd and Cu at 30, 40, 50 and 60°C showed similar kinetics with maximum uptake at 40°C for both Cd and Cu. Chen et al. (1997) investigated the adsorption and desorption of dissolved lead, cadmium and zinc from aqueous solutions using a North Carolina mineral apatite (contaminated soil). Aqueous solutions of Pb, Cd, and Zn were treated with the apatite, followed by desorption experiments under a wide pH conditions ranging from 3 to 12. The adsorption results showed that the apatite was very effective in retaining Pb and was moderately effective for Cd and Zn at pH 4–5. Approximately 100% of the Pb was removed from solutions, representing a capacity of 151 mg of Pb/g of apatite, while 49% of Cd and 29% of Zn added were attenuated, with removal capacities of 73 and 41 mg/g, respectively. The apatite was also effective in removing dissolved Pb, Cd, and Zn leached from the contaminated soil using pH 3–12 solutions by 62.3–99.9, 20–97.9, and 28.6–98.7%, respectively. A summary of different clays and their adsorption capacities for different heavy metal ions is summarized in Table 3.2.
CONCLUSIONS AND RECOMMENDATIONS A wide range of low-cost adsorbents has been studied worldwide for heavy metal removal. It is evident from our literature survey on adsorbents for heavy metals that inexpensive and locally available materials could be used instead of commercial activated carbon. In spite of the scarcity of consistent cost information, the widespread uses of low-cost adsorbents in industries for wastewater treatment applications today are strongly recommended due to their local availability, technical feasibility, engineering applicability, and cost effectiveness. Some low-cost adsorbents such as carbons made from bio-materials and clays have demonstrated outstanding removal capabilities for heavy metals. These adsorbents are efficient and can be effectively used for inorganic effluent treatment containing metal ions. If the alternative adsorbents are found highly efficient for heavy metals removal, not only the industries, but the living organisms and the surrounding environment will also be benefited from the potential toxicity due to heavy metals. Thus, the use of lowcost adsorbents may contribute to the sustainability of the surrounding environment. Undoubtedly low-cost adsorbents offer a lot of promising benefits for commercial purpose in the future.
40
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
NOMENCLATURE aRP: B: b: C0: Ce: Ct: D: E: F: h: I: J: k K: k1: k2: Kc kEL: KEL: KF: kF: kfd: KFS: KH : kip: KL: kr: KRP: Krp: KS: KT : KTh: L: M: m: n: N: P1: P2: P3: P4: P5: P6: qe: qm: qt: R: RL: t: T:
Constant in Redlich-Peterson isotherm model (L/mg1/β) Temkin adsorption model contant (RT/-ΔH) (mg/g) Henry isotherm model (with intercept) constant (mg/g) Initial adsorbate concentration in solution (mg/L) Equilibrium (residual) concentration of adsorbate in solution (mg/L) Adsorbate concentration in solution at time t (mg/L) Dubinin-Radushkevich adsorption model constant (mol2/J2) Mean free energy (J/mol) Fractional attainment of equilibrium (qt/qe) Initial adsorption rate (mg/g-min) Intercept (mg/g) 4-p Fritz – Schluender isotherm model constant (L/g) B-E-T isotherm model constant 4-p Fritz-Schluender isotherm model exponent Pseudo-first-order (Lagergren) adsorption rate constant (min-1) Pseudo-second-order (Ho) adsorption rate constant (g/mg-min) Competitive Langmuir isotherm model constant Extended Langmuir isotherm model constant Extended Langmuir isotherm model constant (L/mg) Freundlich isotherm model constant (L/g) Fractional power kinetic model constant (mg/g) Film diffusion rate constant (min-1) 3-p Fritz – Schluender isotherm model constant (L/mg) Henry isotherm model constant (L/g) Intraparticle diffusion constant (mg/g-min0.5) Langmuir adsorption isotherm model constant (L/mg) Rate constant in Ritchie‟s equation (min-1) Redlich-Peterson isotherm model constant (L/g) Radke-Prausnitz isotherm model constant (L/mg) Sips isotherm model constant (L/g) Temkin isotherm model constant (L/mg) Toth isotherm model constant (L/mg) 4-p Fritz – Schluender isotherm model constant (L/mg) 4-p Fritz – Schluender isotherm model exponent Mass of adsorbent (g) Freundlich adsorption model exponent Sips adsorption model exponent Harkins-Jura model constant (mg/g)2 Harkins-Jura model constant Halsey model constant Halsey model constant Henderson model constant Henderson model exponent Amount of adsorbate adsorbed at equilibrium (mg/g) Maximum adsorption capacity (mg/g) Amount of adsorbate adsorbed at time t (mg/g) Universal gas constant (8.314 J/mol-K) Langmuir separation factor Time (min) Absolute temperature (K)
Carbons and Clays for Heavy Metals Removal …
41
V: Volume of solution (L) Y: Integration constant Greek symbols α: Radke-Prausnitz isotherm model exponent αe: Elovich kinetic model constant (mg/g-min) β: Redlich-Peterson isotherm model exponent βe: Elovich kinetic model constant (g/mg) βr: Ritchie kinetic model constant γ: Sips isotherm model exponent δ: Toth isotherm model exponent ΔH: Heat of adsorption (J) ΔHº: Standard enthalpy change (J) ΔGº: Standard Gibbs energy change (J) ΔSº: Standard entropy change (J/K) ε: Polanyi potential (J/mol) λ: 3-p Fritz – Schluender isotherm model exponent ν: Fractional power model kinetic model exponent (min-1)
LITERATURE CITED Abu-El-Sha‟r WY, Haddad AE. 2007. Lead sorption onto thermally treated soil samples from Irbid. Acta Geotechnica 2, 65-69. Acharya J, Sahu JN, Mohanty CR, Meikap BC. 2009. Removal of lead(II) from wastewater by activated carbon developed from Tamarind wood by zinc chloride activation. Chem Eng J 149, 249-262. Adebowale KO, Unuabonah IE, Olu-Owolabi BI. 2005. Adsorption of some heavy metal ions on sulfate- and phosphate-modified kaolin. Appl Clay Sci 29, 145-148. Aklil A, Mouflih M, Sebti S. 2004. Removal of heavy metal ions from water by using calcined phosphate as a new adsorbent. J Hazard Mater 112, 183-190. Al-Degs YS, El-Barghouthi MI, Issa AA, Khraisheh MA, Walker GM. 2006. Sorption of Zn(II), Pb(II), and Co(II) using natural sorbents: Equilibrium and kinetic studies. Water Res 40, 2645-2658. Al-Jlil SA, Alsewailem FD. 2009. Saudi Arabian clays for lead removal in wastewater. Appl Clay Sci 42, 671-674. Al-Muhtaseb SA, El-Naas MH, Abdallah S. 2008. Removal of aluminum from aqueous solutions by adsorption on date-pit and BDH activated carbons. J Hazard Mater 158, 300-307. Al-Qunaibit MH, Mekhemer WK, Zaghloul AA. 2005. The adsorption of Cu(II) ions on bentonite - a kinetic study. J Colloid Interf Sci 283, 316-321. Altundogan HS, Bahar N, Mujde B, Tumen F. 2007. The use of sulphuric acid-carbonization products of sugar beet pulp in Cr(VI) removal. J Hazard Mater 144, 255-264. Álvarez-Ayuso E, García-Sánchez A. 2003a. Sepiolite as a feasible soil additive for the immobilization of cadmium and zinc. Sci Tot Environ 305, 1-12. Álvarez-Ayuso E, García-Sánchez A. 2003b. Palygorskite as a feasible amendment to stabilize heavy metal polluted soils. Environ Pollut 125, 337-344. Álvarez-Ayuso E, García-Sánchez A. 2007. Removal of cadmium from aqueous solutions by palygorskite. J Hazard Mater 147, 594-600.
42
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
Argun ME. 2008. Use of clinoptilolite for the removal of nickel ions from water: Kinetics and thermodynamics. J Hazard Mater 150, 587-595. Babel S, Kurniawan TA. 2004. Cr(VI) removal from synthetic wastewater using coconut shell charcoal and commercial activated carbon modified with oxidizing agents and/or chitosan. Chemosphere 54, 951-967. Baccar R, Bouzid J, Feki M, Montiel A. 2009. Preparation of activated carbon from Tunisian olive-waste cakes and its application for adsorption of heavy metal ions. J Hazard Mater 162, 1522-1529. Baker HM. 2009. A study of the binding strength and thermodynamic aspects of cadmium and lead ions with natural silicate minerals in aqueous solutions. Desalination 242, 115127. Bansal M, Singh D, Garg VK. 2009. A comparative study for the removal of hexavalent chromium from aqueous solution by agriculture wastes‟ carbons. J Hazard Mater 171, 83-92. Başar CA. 2006. Applicability of the various adsorption models of three dyes adsorption onto activated carbon prepared waste apricot. J Hazard Mater 135, 232-241. Bektaş N, Ağım BA, Kara S. 2004. Kinetic and equilibrium studies in removing lead ions from aqueous solutions by natural sepiolite. J Hazard Mater 112, 115-122. Benhammou A, Yaacoubi A, Nibou L, Tanouti B. 2005a. Adsorption of metal ions onto Moroccan stevensite: kinetic and isotherm studies. J Colloid Interf Sci 282, 320-326. Benhammou A, Yaacoubi A, Nibou L, Tanouti B. 2005b. Study of the removal of mercury(II) and chromium(VI) from aqueous solutions by Moroccan stevensite. J Hazard Mater 117, 243-249. Bhattacharyya KG, Gupta SS. 2006. Adsorption of Fe(III) from water by natural and acid activated clays: Studies on equilibrium isotherm, kinetics and thermodynamics of interactions. Adsorption 12, 185-204. Bhattacharyya KG, Gupta SS. 2007. Adsorptive accumulation of Cd(II), Co(II), Cu(II), Pb(II), and Ni(II) from water on montmorillonite: Influence of acid activation. J Colloid Interf Sci 310, 411-424. Bhattacharyya KG, Gupta SS. 2008. Kaolinite and montmorillonite as adsorbents for Fe(III), Co(II) and Ni(II) in aqueous medium. Appl Clay Sci 41, 1-9. Boyd GE, Adamson AM, Myers LS. 1947. The exchange adsorption of ions from aqueous solutions by organic zeolites. J Am Chem Soc 69, 2836-2848. Brunauer S, Emmett PH, Teller E. 1938. Adsorption of gases in multimolecular layers. J Am Chem Soc 60, 309-319. Cadena F, Rizvi R, Peters RW. 1990. Feasibility studies for the removal of heavy metals from solution using tailored bentonite. In Hazardous and Industrial Wastes, Proceedings of the Twenty-Second Mid-Atlantic Industrial Waste Conference, Drexel University 77-94. Cao X, Ma LQ, Rhue DR, Appel CS. 2004. Mechanisms of lead, copper, and zinc retention by phosphate rock. Environ Pollut 131, 435-444. Chaari I, Fakhfakh E, Chakroun S, Bouzid J, Boujelben N, Feki M, Rocha F, Jamoussi F. 2008. Lead removal from aqueous solutions by a Tunisian smectitic clay. J Hazard Mater 156, 545-551. Chakir A, Bessiere J, Kacemi KEL, Marouf B. 2002. A comparative study of the removal of trivalent chromium from aqueous solutions by bentonite and expanded perlite. J Hazard Mater 95, 29-46.
Carbons and Clays for Heavy Metals Removal …
43
Chantawong V, Harvey NW, Bashkin VN. 2003. Comparison of Heavy Metal Adsorptions by Thai Kaolin and Ballclay. Water Air Soil Pollut 148, 111-125. Chávez-Guerrero L, Rangel-Méndez R, Muñoz-Sandoval E, Cullen DA, Smith DJ, Terrones H, Terrones M. 2008. Production and detailed characterization of bean husk-based carbon: Efficient cadmium (II) removal from aqueous solutions. Water Res 42, 34733479. Chen H, Wang A. 2007. Kinetic and isothermal studies of lead ion adsorption onto palygorskite clay. J Colloid Interf Sci 307, 309-316. Chen H, Zhao Y, Wang A. 2007. Removal of Cu(II) from aqueous solution by adsorption onto acid-activated palygorskite. J Hazard Mater 149, 346-354. Chen X, Wright JV, Conca JL, Peurrung LM. 1997. Evaluation of heavy metal remediation using mineral apatite. Water Air Soil Pollut 98, 57-78. Chien SH, Clayton WR. 1980. Application of Elovich equation to the kinetics of phosphate release and sorption on soils. Soil Sci Soc Am J 44, 265-268. Çoruh S. 2008. The removal of zinc ions by natural and conditioned clinoptilolites. Desalination 225, 41-57. Dalal RC. 1974. Desorption of phosphate by anion exchange resin. Comm Soil Sci Plant Anal 5, 531-538. Demiral H, Demiral İ, Tümsek F, Karabacakoğlu B. 2008. Adsorption of chromium(VI) from aqueous solution by activated carbon derived from olive bagasse and applicability of different adsorption models. Chem Eng J 144, 188-196. Demirbas E, Dizge N, Sulak MT, Kobya M. 2009. Adsorption kinetics and equilibrium of copper from aqueous solutions using hazelnut shell activated carbon. Chem Eng J 148, 480-487. Dho NY, Lee SR. 2003. Effect of Temperature on Single and Competitive Adsorptions of Cu(II) and Zn(II) onto Natural Clays. Environmental Monitoring and Assessment 83, 177-203. Dubinin MM, Radushkevich LV. 1966. Evaluation of microporous materials with a new isotherm. Dokl Akad Nauk SSSR 55, 331-333. Eren E. 2008. Removal of copper ions by modified Unye clay, Turkey. J Hazard Mater 159, 235-244. Eren E, Afsin B. 2008. An investigation of Cu(II) adsorption by raw and acid-activated bentonite: A combined potentiometric, thermodynamic, XRD, IR, DTA study. J Hazard Mater 151, 682-691. Fahim NF, Barsoum BN, Eid AE, Khalil MS. 2006. Removal of chromium(III) from tannery wastewater using activated carbon from sugar industrial waste. J Hazard Mater 136, 303309. Fonseca MG, Oliveira MM, Arakaki LNH. 2006. Removal of cadmium, zinc, manganese and chromium cations from aqueous solution by a clay mineral. J Hazard Mater 137, 288292. Freundlich H. 1907. Über die adsorption in lösungen. Z Phys Chem 57, 385-470. Fritz W, Schluender EU. 1974. Simultaneous adsorption equilibria of organic solutes in dilute aqueous solution on activated carbon. Ceram Eng Sci Proc 29, 1279-1282. Gerçel Ö, Gerçel HF. 2007. Adsorption of lead(II) ions from aqueous solutions by activated carbon prepared from biomass plant material of Euphorbia rigida. Chem Eng J 132, 289297.
44
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
Ghorbel-Abid I, Jrad A, Nahdi K, Trabelsi-Ayadi M. 2009. Sorption of chromium (III) from aqueous solution using bentonitic clay. Desalination 246, 595-604. Ghosh PK. 2009. Hexavalent chromium [Cr(VI)] removal by acid modified waste activated carbons. J Hazard Mater 171, 116-122. Guerra DL, Viana RR, Airoldi C. 2009. Application of natural and modified hectorite clays as adsorbents to removal of Cr(VI) from aqueous solution–Thermodynamic and equilibrium study. J Hazard Mater 172, 507-514. Günay A, Arslankaya E, Tosun İ. 2007. Lead removal from aqueous solution by natural and pretreated clinoptilolite: Adsorption equilibrium and kinetics. J Hazard Mater 146, 362371. Gupta SS, Bhattacharyya KG. 2006. Adsorption of Ni(II) on clays. J Colloid Interf Sci 295, 21-32. Gürü M, Venedik D, Murathan A. 2008. Removal of trivalent chromium from water using low-cost natural diatomite. J Hazard Mater 160, 318-323. Hall KR, Eagleton LC, Acrivos A, Vermeulen T. 1966. Pore and solid diffusion kinetics in fixed-bed adsorption under constant pattern conditions. Ind Eng Chem Fundam 5, 212223. Halsey G. 1948. Physical adsorption on non-uniform surfaces. J Chem Phys 16, 931-937. Hasar H. 2003. Adsorption of nickel(II) from aqueous solution onto activated carbon prepared from almond husk. J Hazard Mater 97, 49-57. Hayward DO, Trapnell BMW. 1964. Chemisorption. 2nd Ed., Butterworth, London. Henderson SM. 1952. A basic concept of equilibrium moisture. Agric Eng 33, 29-32. Ho YS. 2004a. Selection of optimum sorption isotherm. Carbon 42, 2115-2116. Ho YS. 2004b. Citation review of Lagergren kinetic rate equation on adsorption reactions. Scientometrics 59, 171-177. Ho YS. 2006a. Review of second-order models for adsorption systems. J Hazard Mater 136, 681-689. Ho YS. 2006b. Second-order kinetic model for the sorption of cadmium onto tree fern: A comparison of linear and non-linear methods. Water Res 40, 119-125. Ho YS, McKay G. 1999. Pseudo-second order model for sorption processes. Process Biochem 34, 451-465. Ho YS, McKay G. 2000. Correlative biosorption equilibria model for binary batch system. Chem Eng Sci 55, 817-825. Ho YS, Ofomaja AE. 2005. Kinetics and thermodynamics of lead ion biosorption on palm kernel fibre from aqueous solution. Process Biochem 40, 3455-3461. Ho YS, Ofomaja AE. 2006. Biosorption thermodynamics of cadmium on coconut copra meal as biosorbent. Biochem Eng J 30, 117-123. Hsu NH, Wang SL, Liao YH, Huang ST, Tzou YM, Huang YM. 2009. Removal of hexavalent chromium from acidic aqueous solutions using rice straw-derived carbon. J Hazard Mater 171, 1066-1070. Imamoglu M, Tekir O. 2008. Removal of copper (II) and lead (II) ions from aqueous solutions by adsorption on activated carbon from a new precursor hazelnut husks. Desalination 228, 108-113. Issabayeva G, Aroua MK, Sulaiman NMN. 2006. Removal of lead from aqueous solutions on palm shell activated carbon. Bioresour Technol 97, 2350-2355.
Carbons and Clays for Heavy Metals Removal …
45
Jiang MQ, Wang QP, Jin XY, Chen ZL. 2009. Removal of Pb(II) from aqueous solution using modified and unmodified kaolinite clay. J Hazard Mater 170, 332-339. Kadirvelu K, Faur-Brasquet C, Le Cloirec P. 2000. Removal of Cu (II), Pb (II) and Ni (II) by adsorption onto activated carbon cloths. Langmuir 16, 8404-8409. Kadirvelu K, Senthilkumar P, Thamaraiselvi K, Subburam V. 2002. Activated carbon prepared from biomass as adsorbent: elimination of Ni(II) from aqueous solution. Bioresour Technol 81, 87-90. Kannan N, Rengasamy G. 2005. Comparison of cadmium ion adsorption on various activated carbons. Water Air Soil Pollut 2005, 185-201. Karthikeyan T, Rajgopal S, Miranda LR. 2005. Chromium(VI) adsorption from aqueous solution by Hevea Brasilinesis sawdust activated carbon. J Hazard Mater 124, 192-199. Khamis M, Jumean F, Abdo N. 2009. Speciation and removal of chromium from aqueous solution by white, yellow and red UAE sand. J Hazard Mater 169, 948-952. Kobya M, Demirbas E, Senturk E, Ince M. 2005. Adsorption of heavy metal ions from aqueous solutions by activated carbon prepared from apricot stone. Bioresour Technol 96, 1518-1521. Kortenkamp A, Casadevall M, Faux SP, Jenner A, Shayer ROJ, Woodbridge N, O‟Brien P. 1996. A role for molecular oxygen in the formation of DNA damage during the reduction of the carcinogen Cr(VI) by glutathione. Arch Biochem Biophys 329, 199-208. Krishnan KA, Anirudhan TS. 2008. Kinetic and equilibrium modelling of cobalt(II) adsorption onto bagasse pith based sulphurised activated carbon. Chem Eng J 137, 257264. Kubilay Ş, Gürkan R, Savran A, Şahan T. 2007. Removal of Cu(II), Zn(II) and Co(II) ions from aqueous solutions by adsorption onto natural bentonite. Adsorption 13, 41-51. Kula I, Uğurlu M, Karaoğlu H, Çelik A. 2008. Adsorption of Cd(II) ions from aqueous solutions using activated carbon prepared from olive stone by ZnCl2 activation. Bioresour Technol 99, 492-501. Kwon JS, Yun ST, Kim SO, Mayer B, Hutcheon I. 2005. Sorption of Zn(II) in aqueous solutions by scoria. Chemosphere 60, 1416-1426. Lagadic IL, Mitchell MK, Payne BD. 2001. Highly Effective Adsorption of Heavy Metal Ions by a Thiol-Functionalized Magnesium Phyllosilicate Clay. Environ Sci Technol 35, 984990. Lagergren S. 1898. About the theory of so-called adsorption of soluble substances. K Sven Vetenskapsakad Handlingar Band 24, 1-39. Lalhruaitluanga H, Jayaram K, Prasad MNV, Kumar KK. 2009. Lead(II) adsorption from aqueous solutions by raw and activated charcoals of Melocanna baccifera Roxburgh (bamboo) - A comparative study. J Hazard Mater 175, 311-318. Langmuir I. 1916. The constitution and fundamental properties of solids and liquids. I. solids. J Am Chem Soc 38, 2221-2295. Langmuir I. 1917. The constitution and fundamental properties of solids and liquids. II. Liquids. J Am Chem Soc 39, 1848-1906. Langmuir I. 1918. The adsorption of gases on plane surfaces of glass, mica and platinum. J Am Chem Soc 40, 1361-1403. Lata H, Garg VK, Gupta RK. 2008. Sequestration of nickel from aqueous solution onto activated carbon prepared from Parthenium hysterophorus L. J Hazard Mater 157, 503509.
46
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
Li K, Wang X. 2009. Adsorptive removal of Pb(II) by activated carbon prepared from Spartina alterniflora: Equilibrium, kinetics and thermodynamics. Bioresour Technol 100, 2810-2815. Low MJD. 1960. Kinetics of chemisorption of gases on solids. Chem Rev 60, 267-312. Malandrino M, Abollino O, Giacomino A, Aceto M, Mentasti E. 2006. Adsorption of heavy metals on vermiculite: Influence of pH and organic ligands. J Colloid Interf Sci 299, 537546. Manohar DM, Noeline BF, Anirudhan TS. 2005. Removal of Vanadium(IV) from Aqueous Solutions by Adsorption Process with Aluminum-Pillared Bentonite. Ind Eng Chem Res 44, 6676-6684. Manohar DM, Noeline BF, Anirudhan TS. 2006. Adsorption performance of Al-pillared bentonite clay for the removal of cobalt(II) from aqueous phase. Appl Clay Sci 31, 194206. McKay G, Otterburn MS, Aga JA. 1987. Intraparticle diffusion process occurring during adsorption of dyestuffs. Water Air Soil Pollut 36, 381-390. Mohan D, Singh KP. 2002. Single- and multi-component adsorption of cadmium and zinc using activated carbon derived from bagasse – an agricultural waste. Water Res 36, 23042318. Mohan D, Singh KP, Singh VK. 2006. Trivalent chromium removal from wastewater using low cost activated carbon derived from agricultural waste material and activated carbon fabric cloth. J Hazard Mater 135, 280-295. Monser L, Adhoum N. 2009. Tartrazine modified activated carbon for the removal of Pb(II), Cd(II) and Cr(III). J Hazard Mater 161, 263-269. Mouflih M, Aklil A, Sebti S. 2005. Removal of lead from aqueous solutions by activated phosphate. J Hazard Mater 119, 183-188. Nadeem M, Shabbir M, Abdullah MA, Shah SS, McKay G. 2009. Sorption of cadmium from aqueous solution by surfactant-modified carbon adsorbents. Chem Eng J 148, 365-370. Namasivayam C, Kadirvelu K. 1999. Uptake of mercury (II) from wastewater by activated carbon from unwanted agricultural solid waste by-product: coir pith. Carbon 37, 79-84. Namasivayam C, Periasamy K. 1993. Bicarbonate-treated peanut hull carbon for mercury (II) removal from aqueous solution. Water Res 27, 1663-1668. Nemr AE. 2009. Potential of pomegranate husk carbon for Cr(VI) removal from wastewater: Kinetic and isotherm studies. J Hazard Mater 161, 132-141. Nemr AE, Khaled A, Abdelwahab O, El-Sikaily A. 2008. Treatment of wastewater containing toxic chromium using new activated carbon developed from date palm seed. J Hazard Mater 152, 263-275. Oubagaranadin JUK, Murthy ZVP. 2009a. Removal of Pb(II) from aqueous solutions by carbons prepared from Sal wood (Shorea robusta). Eur J Wood Prod 67, 197-206. Oubagaranadin JUK, Murthy ZVP. 2009b. Modeling of adsorption of Cr(VI) on activated carbons derived from corn (Zea Mays) cob. Chemical Product and Process Modeling 4, Article 32. Oubagaranadin JUK, Murthy ZVP. 2009c. Adsorption of divalent lead on a montmorillonite – illite type of clay. Ind Eng Chem Res 48, 10627-10636. Oubagaranadin JUK, Murthy ZVP. 2010. Characterization and use of acid-activated montmorillonite-illite type of clay for lead(II) removal. AIChE J 56, 2312-2322.
Carbons and Clays for Heavy Metals Removal …
47
Oubagaranadin JUK, Sathyamurthy N, Murthy ZVP. 2007. Evaluation of Fuller‟s earth for the adsorption of mercury from aqueous solutions: A comparative study with activated carbon. J Hazard Mater 142, 165-174. Owlad M, Aroua MK, Daud WMAW. 2010. Hexavalent chromium adsorption on impregnated palm shell activated carbon with polyethyleneimine. Bioresour Technol 101, 5098-5103. Özçimen D, Ersoy-Meriçboyu A. 2009. Removal of copper from aqueous solutions by adsorption onto chestnut shell and grapeseed activated carbons. J Hazard Mater 168, 1118-1125. Pehlivan E, Cetin S, Yanik BH. 2006. Equilibrium studies for the sorption of zinc and copper from aqueous solutions using sugar beet pulp and fly ash. J Hazard Mater 135, 193-199. Radke CJ, Prausnitz JM. 1972. Adsorption of organic solutes from dilute aqueous solution of activated carbon. Ind Eng Chem Fundamn 11, 445-451. Rao MM, Ramana DK, Seshaiah K, Wang MC, Chien SWC. 2009. Removal of some metal ions by activated carbon prepared from Phaseolus aureus hulls. J Hazard Mater 166, 1006-1013. Rao MM, Ramesh A, Rao GPC, Seshaiah K. 2006. Removal of copper and cadmium from the aqueous solutions by activated carbon derived from Ceiba pentandra hulls. J Hazard Mater 129, 123-129. Rashed MN. 2001. Lead removal from contaminated water using mineral adsorbents. The Environmentalist 21, 187-195. Redlich O, Peterson DL. 1959. A useful adsorption isotherm. J Phys Chem 63, 1024-1026. Ritchie AG. 1977. Alternative to the Elovich equation for the kinetics of adsorption of gases on solids. J Chem Soc, Faraday Trans I 73, 1650-1653. Rosene MR, Manes M. 1977. Application of the Polanyi adsorption potential theory to adsorption from solution on activated carbon. J Phys Chem 81, 1651-1657. Rudzinski W, Plazinski W. 2006. Kinetics of solute adsorption at solid/solution interfaces: A theoretical development of the empirical pseudo-first and pseudo-second order kinetic rate equations, based on applying the statistical rate theory of interfacial transport. J Phys Chem B 110, 16514-16525. Sag Y, Kutsal T. 2000. Determination of the biosorption activation energies of heavy metal ions on Zoogloea ramigera and Rhizopus arrhizus. Process Biochem 35, 801-807. Santos ACV, Masini JC. 2007. Evaluating the removal of Cd(II), Pb(II) and Cu(II) from a wastewater sample of a coating industry by adsorption onto vermiculite. Appl Clay Sci 37, 167-174. Sari A, Tuzen M, Citak D, Soylak M. 2007. Equilibrium, kinetic and thermodynamic studies of adsorption of Pb(II) from aqueous solution onto Turkish kaolinite clay. J Hazardous Mater 149, 283-291. Sarioglu M, Atay ÜA, Cebeci Y. 2005. Removal of copper from aqueous solutions by phosphate rock. Desalination 181, 303-311. Satapathy D, Natarajan GS. 2006. Potassium bromate modification of the granular activated carbon and its effect on nickel adsorption. Adsorption 12, 147-154. Sekar M, Sakthi V, Rengaraj S. 2004. Kinetics and equilibrium adsorption study of lead(II) onto activated carbon prepared from coconut shell. J Colloid Interf Sci 279, 307-313. Selvi K, Pattabhi S, Kadirvelu K. 2001. Removal of Cr(VI) from aqueous solution by adsorption onto activated carbon. Bioresour Technol 80, 87-89.
48
John U. Kennedy Oubagaranadin and Z.V.P. Murthy
Seng CE, Lee CG, Liew KY. 2001. Adsorption of chromium(VI) and nickel(II) ions on acidand heat-activated deoiled spent bleaching clay. Journal of the American Oil Chemist’s Society 78, 831-835. Sharma YC, Kaul SN, Weng CH. 2007. Adsorptive separation of cadmium from aqueous solutions and wastewaters by riverbed sand. Environ Pollut 150, 251-257. Shawabkeh RA, Al-Khashman OA, Al-Omari HS, Shawabkeh AF. 2007. Cobalt and zinc removal from aqueous solution by chemically treated bentonite. The Environmentalist 27, 357-363. Singh CK, Sahu JN, Mahalik KK, Mohanty CR, Raj Mohan B, Meikap BC. 2008. Studies on the removal of Pb(II) from wastewater by activated carbon developed from Tamarind wood activated with sulphuric acid. J Hazard Mater 153, 221-228. Sips R. 1948. On the structure of a catalyst surface. J Chem Phys 16, 490-495. Ńljivić M, Smičiklas I, Pejanović S, Plećań I. 2009. Comparative study of Cu2+ adsorption on a zeolite, a clay and a diatomite from Serbia. Appl Clay Sci 43, 33-40. Smith JM, Van Ness HC. 1987. Introduction to chemical engineering thermodynamics. 4th Ed., McGraw Hill, Singapore. Sparks DL. 1986. Kinetics of reaction in pure and mixed systems. In: Sparks DL (Editor). Soil physical chemistry. Boca Raton, CRC Press. Sprynskyy M, Buszewski B, Terzyk AP, Namieśnik J. 2006. Study of the selection mechanism of heavy metal (Pb2+, Cu2+, Ni2+, and Cd2+) adsorption on clinoptilolite. J Colloid Interf Sci 304, 21-28. Srivastava P, Singh B, Angove M. Prashant S, Balwant S, Michael A. 2005. Competitive adsorption behavior of heavy metals on kaolinite. J Colloid Interf Sci 290, 28-38. Suraj G, Iyer CSP, Lalithambika M. 1998. Adsorption of cadmium and copper by modified kaolinites. Appl Clay Sci 13, 293-306. Tajar AF, Kaghazchi T, Soleimani M. 2009. Adsorption of cadmium from aqueous solutions on sulfurized activated carbon prepared from nut shells. J Hazard Mater 165, 1159-1164. Temkin MJ, Pyzhev V. 1940. Recent modifications to Langmuir isotherms. Acta Physicochim URSS 12, 217-225. Tóth J. 2000. Calculation of the BET-compatible surface area from any Type I isotherms measured above the critical temperature. J Colloid Interf Sci 225, 378-383. Treybal RE. 1981. Mass-Transfer Operations. 3rd Ed., McGraw Hill, Tokyo. Turan P, Doğan M, Alkan M. 2007. Uptake of trivalent chromium ions from aqueous solutions using kaolinite. J Hazard Mater 148, 56-63. Unuabonah EI, Adebowale KO, Olu-Owolabi BI, Yang LZ. 2008a. Comparison of sorption of Pb2+ and Cd2+ on Kaolinite clay and polyvinyl alcohol-modified Kaolinite clay. Adsorption 14, 791-803. Unuabonah EI, Adebowale KO, Olu-Owolabi BI, Yang LZ, Kong LX. 2008b. Adsorption of Pb (II) and Cd (II) from aqueous solutions onto sodium tetraborate-modified Kaolinite clay: Equilibrium and thermodynamic studies. Hydrometallurgy 93, 1-9. Veli S, Alyüz B. 2007. Adsorption of copper and zinc from aqueous solutions by using natural clay. J Hazard Mater 149, 226-233. Vengris T, Binkiené R, Sveikauskaité A. 2001. Nickel, copper and zinc removal from waste water by a modified clay sorbent. Appl Clay Sci 18, 183-190.
Carbons and Clays for Heavy Metals Removal …
49
Vieira MGA, Almeida Neto AF, Gimenes ML, da Silva MGC. 2010. Sorption kinetics and equilibrium for the removal of nickel ions from aqueous phase on calcined Bofe bentonite clay. J Hazard Mater 177, 362-371. Wang FY, Wang H, Ma JW. 2010. Adsorption of cadmium (II) ions from aqueous solution by a new low-cost adsorbent - Bamboo charcoal. J Hazard Mater 177, 300-306. Wang S, Dong Y, He M, Chen L, Yu X. 2009. Characterization of GMZ bentonite and its application in the adsorption of Pb(II) from aqueous solutions. Appl Clay Sci 43, 164171. Weber Jr. WJ, Morris JC. 1963. Kinetics of adsorption on carbon from solution. J Sanitary Eng Div: Am Soc Civil Eng 89, SA2, 31-60. Weng CH, Sharma YC, Chu SH. 2008. Adsorption of Cr(VI) from aqueous solutions by spent activated clay. J Hazard Mater 155, 65-75. Wilson K, Yang H, Seo CW, Marshall WE. 2006. Select metal adsorption by activated carbon made from peanut shells. Bioresour Technol 97, 2266-2270. Yao C. 2000. Extended and Improved Langmuir Equation for Correlating Adsorption Equilibrium Data. Sep Purif Technol 19, 237-242. Yavuz Ö, Altunkaynak Y, Güzel F. 2003. Removal of copper, nickel, cobalt and manganese from aqueous solution by kaolinite. Water Res 37, 948-952. Zabihi M, Asl AH, Ahmadpour A. 2009. Removal of mercury from water by carbonaceous sorbents derived from walnut shell. J Hazard Mater 167, 230-236. Zaini MAA, Okayama R, Machida M. 2009. Adsorption of aqueous metal ions on cattlemanure-compost based activated carbons. J Hazard Mater 170, 1119-1124. Zhu S, Hou H, Xue Y. 2008. Kinetic and isothermal studies of lead ion adsorption onto bentonite. Appl Clay Sci 40, 171-178.
In: Langmuir Monolayers … Editor: Jennifer A. Sherwin
ISBN: 978-1-61122-461-0 ©2011 Nova Science Publishers, Inc.
Chapter 2
MOLECULAR ORGANIZATION OF THERMOTROPIC LIQUID CRYSTALS AND THEIR MIXTURES WITH AZO DYES IN LANGMUIR AND LANGMUIR-BLODGETT FILMS Danuta Bauman, Anna Modlińska and Krzysztof Inglot Faculty of Technical Physics, Poznań University of Technology, Poznań, Poland
ABSTRACT In this review article the results of the study of thermotropic liquid crystals and of binary mixtures of dichroic azo dye/liquid crystal in Langmuir and Langmuir-Blodgett films are presented. The liquid crystals of rod-like shape from various homologous series and nine azo dyes with different molecular structure as well as different values and directions of the dipole moment were chosen. It was found that the liquid crystals with the terminal isothiocyanato (–NCS) group are not able to form a compressible monolayer at the water surface. Very short and very long alkyl or alkoxy chains attached to the rigid molecular core also hinder the creation of the stable film. Azo dyes cannot form the Langmuir film themselves; therefore, the liquid crystals 4-n-octyl-4'-cyanobiphenyl (8CB) and trans-4-n-octyl(4‟-cyanophenyl)-hexane (8PCH) were used as supporting matrices. The Langmuir films were characterized by the surface pressure-area and surface potential-area isotherms and by Brewster angle microscopy (BAM). The analysis of the isotherms and BAM images of liquid crystals indicated that the organization of the mesogenic molecules at the air-water interface is dependent on their structure and to some extent reflects their ability to form an appropriate mesophase in the bulk. For the binary azo dye/8CB mixtures the miscibility of two components as well as the organization and the packing of molecules at the water surface were determined. The absorption spectra by using natural and linearly polarized light were recorded for both Langmuir and Langmuir-Blodgett films. Information about spectral properties of ultrathin layers and ability of dye and liquid crystal molecules to form self-aggregates was obtained. The polarized absorption spectra allowed one to determine the alignment of molecules on the quartz surface.
52
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
1. INTRODUCTION In the XXI century, modern electronic devices tend to increasing miniaturization. The smaller the system, the faster and more economically it can work. Unfortunately, it is more and more difficult and expensive to produce it. Difficulties arise, among other things, because of the non-applicability of classical physics laws at the atomic scale. Indeed it is expected that some progress towards miniaturization could yet be made using three-dimensional (3D) systems, but it is necessary to work more diligently on the use of single molecules or small molecular aggregates as functionalizing materials in electronic devices. Various nanotechnologies come here with the help – it is searching for quick, reliable and economically efficient methods which will produce systems on the nanoscale. The LangmuirBlodgett (LB) method is considered as one of the most versatile techniques currently used worldwide to produce nanostructures. As this is a unique technique that allows us to create two-dimensional (2D) ordered layers of certain molecules or colloidal particles, the architecture of which can be manipulated with ease, there exists good opportunity to optimize the physical parameters (mainly electro-optical) of the material used. Thus, LB films are now an integral part of a knowledge area related to the molecular electronics [1]. LB film properties depend strongly on the properties of a Langmuir film; therefore, it is necessary to study comprehensively both types of films. Stable monolayers at gas-liquid (Langmuir films) and gas-solid (LB films) interfaces are generally formed by amphiphilic molecules; thus, it is not astonishing that they can be formed of lyotropic liquid crystals. Thermotropic liquid crystal molecules cannot be directly treated as amphiphilic, nevertheless many of them are able to create stable and compressible monolayers at the liquid surface, which can be next transferred at the solid substrates [2]. Already in the eighties and nineties of the last century, it was found that some thermotropic liquid crystals with rod-like shaped molecules possessing strongly polar hydrophilic head group and hydrophobic alkyl chain can form stable 2D monolayers at the air-water interface, which can be transferred onto the solid substrates [3-7]. Such monolayers are very simple systems, in which the intermolecular interactions can be investigated [1,8]. Moreover, studying Langmuir and LB films formed from liquid crystals, it is possible to obtain information about the way in which the molecules are anchored to the interface, and how these interfacial interactions affect the macroscopic molecular alignment in the bulk. Thermotropic liquid crystals can also be used, likewise fatty acids, as supporting matrices for compounds which are not able to form compressible and stable monolayers at the liquid surface themselves. They were used, e.g., to support molecules of various azo dyes, and stable Langmuir and LB films of azo dye/liquid crystal mixtures were obtained and investigated [917]. The opportunity to study the properties of azo dyes in Langmuir and LB films is very essential due to the strong tendency to formation of self-aggregates by molecules of these compounds. In films fabricated by using LB technique, molecules are in a highly ordered environment, similarly as in solid matrices, where aggregation of aromatic molecules is frequently observed [17]. Interest in molecular aggregates has grown in recent years because of intriguing optical properties of these systems, giving the possibility to use them as modern functional materials, both in the field of molecular electronics and photonics. Moreover, azo dyes are characterized by the large change of the dipole moment at * transition, and thus
Molecular Organization of Thermotropic Liquid Crystals …
53
by a high value of hyperpolarizability. Therefore, incorporated into highly oriented matrices, they can find application in nonlinear optics [19]. In this review article, the results of the study of 2D layers formed of thermotropic liquid crystals and of binary mixtures of dichroic azo dye/liquid crystal at the air-water and airquartz interfaces are presented. The liquid crystals of rod-like shaped molecules from various homologous series were investigated. The aim of our study was to recognize the relationship between the structure of mesogenic molecules and stability of monolayers formed by them at interfaces. We also tried to explore to what extent only the orientational order in the nematic phase, and both the orientational and positional orders leading to the layered structure in the smectic phase, are preserved if we consider a liquid crystal layer with a thickness of the order of the molecular dimension. Next, two liquid crystals, 4-n-octyl-4‟-cyanobiphenyl (8CB) and trans-4-n-octyl(4‟-cyanophenyl)-hexane (8PCH) were chosen as supporting matrices for nine azo dyes with different molecular structure. We would like to know the effect of the structure as well as the value and the direction of the dipole moment of dye molecules on their polar ordering and the tendency to creation of self-aggregates in Langmuir and LB films. Table 1. Molecular structure of liquid crystals investigated. Abbreviation
Molecular structure
n for compounds investigated
nCB
4–9
nPCH
4 – 10
nOCB
2 – 14
nCPB
2 – 12
nCHBT
3–9
nBOBT
5–8
8OCFPB
8
8OCPFB
8
54
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
2. EXPERIMENTAL The thermotropic rod-shaped (calamitic) liquid crystals often used as components for preparation of mixtures for liquid crystal displays (LCDs) were studied. The molecular structure of these liquid crystals is seen in Table 1. All compounds were synthesized and chromatographically purified at the Institute of Chemistry, Military University of Technology, Warsaw (Poland). The most of the liquid crystals under investigation has only nematic (N) phase between solid and isotropic phases. Some of them, as for example 8CB, 9CB, 8OCB, 9OCB, have both nematic and smectic A (SmA) phases, while some as 10CB or 12PCH show only SmA phase. The molecular structure of the dyes used is presented in Table 2. All the dyes were synthesized and chromatographically purified in Institute of Polymer Technology and Dyes at Łódź University of Technology, Poland. A commercially available Minitrough 2 Langmuir-Blodgett system (KSV Instruments Ltd., Finland) was used for fabrication of spread monolayers on the water surface and for LB films deposition. Ultrapure water characterized by resistivity of 18.2 M·cm, used as a subphase in the trough, was destilled and passed through a Milli-Q water purification system. The liquid crystals and azo dyes were first dissolved in chloroform (Uvasol, for spectroscopy, E. Merck) at a concentration of 0.1 mM in order to obtain stock solutions and kept refrigerated. The concentration of solutions was confirmed spectroscopically. The dye/liquid crystal mixture solutions were made at a constant concentration of the liquid crystal (0.3 g/l) and appropriate amounts of the dye to obtain the molar fraction (XM) of the dye in the whole range of possible concentrations (depending on the dye solubility). The solution of the appropriate liquid crystal or dye/liquid crystal mixture was then spread drop by drop from a microlitre syringe (Hamilton, England) onto the subphase to form a monolayer and was equilibrated for about 15 minutes to allow the chloroform to evaporate. Then the floating monolayer was slowly compressed, symmetrically from both sides at a barrier motion speed of 5 mm min-1. All measurements were repeated on fresh subphases three to five times to confirm reproducibility. Standard trough cleaning procedure was adopted between measurements. A constant subphase temperature was maintained by a cooling circulator and kept constant at (210.5)oC. Additionally, some experiments for liquid crystal 8CB were made at different temperatures, up to 45oC. The most basic characterization of Langmuir films is the measurement of the surface pressure versus the average area available for one molecule isotherm (-A isotherm) [1,8]. For monolayers, is defined as the surface tension of the pure subphase minus the surface tension of the subphase-monolayer system. In our experiment the surface pressure was monitored by a platinium Wilhelmy plate balance with an accuracy of 0.1 mN/m. Additionally, the surface potential (V) of the monolayer as a function of the mean molecular area (V-A isotherm) was measured using the vibrating plate method by means of a SPOT 1 head from KSV. An accuracy of this method was 1.0 mV. V is defined as the difference in the potential between a monolayer-covered surface and a clean subphase surface [8] and can be related to an average effective dipole moment for monolayer-forming molecules by Helmholtz equation [20,21]:
Molecular Organization of Thermotropic Liquid Crystals …
V
, A r 0
55
(1)
Table 2. Molecular structure of dyes investigated. Compound
Molecular structure
1
2
3
4
5
6
7
8
9
where = cos is the average vertical component of the molecular dipole moment, is the angle between the surface normal and the dipole axis, and r and 0 are the dielectric constant of the monolayer and the electric permittivity of the free space, respectively.
56
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
The morphology of the films at the air-water interface was monitored by means of a Brewster angle microscope (BAM). The instrument we used is based on Hoenig and Moebius setup [22] and was built in our laboratory [14]. The green (532 nm) laser beam was directed at the Brewster angle (53.1o) onto the pure water. The light reflected from the monolayer was imaged by means of a CCD camera. The BAM images obtained were recorded directly on the hard disc of PC computer both on the continuous slow film compression and expansion, simultaneously with the isotherm record. Typical reproducible images for the films at various surface pressures were saved in files using a framegraber and printed. The image features were observed with a lateral resolution of 5 m. Absorption spectra of spread monolayers on the water surface were recorded in situ by means of a spectrophotometer Varian CARY 400 equipped with fiber optic accessory supplied by Varian. The quartz fiber bundle delivered UV and Vis radiation from appropriate lamps in the spectrophotometer to the Langmuir film on a trough with a quartz window at the center. Another bundle collected the light transmitted trough the film and led it back to the spectrophotometer (detector) sample compartment. Both fiber bundles were fixed in the holder, which enabled us to position the end of the bundle vertically to the water surface on both sides of the trough. The fiber bundles were precisely focused on the film to maximalize the transmitted light level. The reference light beam of the spectrophotometer was properly attenuated to reduce a level of noise. Stability tests were done for the Langmuir films to keep the pressure constant and LB films were fabricated using electronically controlled dipping device. The substrates for LB films were polished quartz plates (35x10x1mm3) with hydrophilic surfaces. The dipper speed was ca. 5 mm/min, and the dipping stroke was 25 mm. Langmuir films were transferred onto both sides of quartz slides at the surface pressure below the collapse point, which corresponds to the stage of the formation of the compressed monolayer. The transfer ratio (TR), defined as the ratio of the actual decrease in the subphase area to the actual area on the substrate coated by the floating layer, was estimated to be between 1.0 and 1.2. The deposition of the Langmuir film of the compounds under investigation onto the quartz was successful only at raising the substrate. Repeated attempts to transfer a floating layer onto quartz slides failed. Therefore, only one dipping and one raising were made.
Figure 1. Geometry for the polarized absorption measurements.
EP and ES
are the electric vectors of
the incident light polarized, respectively, parallel and perpendicularly to the plane of incidence. is the incidence angle. AP and AS are components of absorbance.
Molecular Organization of Thermotropic Liquid Crystals …
57
The absorption spectra of LB films were recorded in the UV-Vis region by means of a spectrophotometer CARY 400, equipped with an angular sample holder. The measurements were performed in the geometry presented in Fig. 1. Both natural and linearly polarized light were used. The incident light beam was normal to the substrate surface by using natural light, whereas polarized spectra were recorded at the incidence angle = 0o, 30o and 60o. In order to obtain the polarized light, the Glan-Thomson polarizers were used.
3. RESULTS AND DISCUSSION 3.1. Langmuir and Langmuir-Blodgett Films of Liquid Crystals 3.1.1. Langmuir Film Characterization The amphiphilic character of rod-shaped liquid crystal molecules is not sufficient condition for the formation of stable and compressible monolayers at the air-water interface. From our study follows that all the members of the homologous series of 4-(trans-4‟-nalkylcyclohexyl)-isothiocyanato-benzene (nCHBT), and n-alkyl-4-(4‟-isothiocyanatophenyl)bicyclo[2,2,2]-octanes (nBOBT) give monolayers which are unable to offer any significant resistance to barrier compression. All these compounds have the terminal –NCS group and it seems that already this group causes the formation of the Langmuir film impossible. The other liquid crystals under investigation have the terminal –CN group. Among them only those with very short and very long alkyl or alkoxy chain could not form a stable monolayer [14,23,24]. The most comprehensive investigations were carried out for the liquid crystal 4-n-octyl4‟-cyanobiphenyl (8CB) in the Langmuir film and the results can be found in references [3,57,14,23-26]. Figure 2 illustrates the dependence of the surface pressure, , on the average area available for one molecule, A, while compressing and expanding the monolayer of 8CB on the water surface. The expansion isotherm shows only slight hysteresis, which means that the equilibrium conditions were obtained. Following Xue et al. [5] we can distinguish in the measured area range five regions. In the region where the mean molecular area is greater than 0.50 nm2 (region I), is near to zero and constant, which indicates the coexistence of gas and liquid phases. Between 0.48 and 0.41 nm2 (region II), the first significant increase in up to the collapse point occurs (the collapse point is recognized as the point in the -A isotherm where the ratio /A begins to decrease due to the next phase transition), indicating the formation of the completely homogeneous monolayer. However, the collapse point occurs at the mean molecular area larger by a factor of two than the theoretical molecular cross-section. This effect was explained in terms of strong repulsive interactions between the electric dipoles of the cyano groups. As a result of such interactions, the 8CB monolayer is fragile, molecules are not densely packed and are tilted to the water surface. By further compression of the 8CB film (region III), the plateau region is observed: remains constant with decreasing the A value. When A reaches about 0.11 nm2 (region IV), rises sharply. This value is too small for all the molecules to remain on the water surface and therefore it was postulated that in this A region an interdigitated bilayer on the top of the monolayer (trilayer) is created [5,6]. After further compression (region V) a second plateau appears suggesting the creation of the uniform multilayer.
58
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
Figure 2. Surface pressure-area isotherms of 8CB Langmuir film recorded during compression and expansion processes [23] with schematic representation of molecular alignment in various stages of the film formation.
Figure 3. Surface pressure-area isotherms of Langmuir films formed of representative liquid crystals with n = 8.
Figure 3 presents -A isotherms obtained during compression process for members with n = 8 for series investigated. With a decrease of the available area, the surface pressure rises up to the collapse point, indicating the formation of the compressed monolayer. In the case of the liquid crystals 8CB, 8PCH (trans-4-n-octyl(4‟-cyanophenyl)-hexane) and 8OCFPB (4-
Molecular Organization of Thermotropic Liquid Crystals …
59
cyano-3-fluorophenyl 4‟-n-octyloxybenzoate), behind the collapse point in the -A isotherms a broad plateau is observed, and it was found that the expansion isotherms show only a slight hysteresis with respect to the compression ones. This implies that the films created are very stable. In the case of the liquid crystals 8OCB (4-n-octyloxy-4‟-cyanobiphenyl), 8CPB (4-nalkyl(4‟-cyanophenyl)benzoate) and 8OCPFB (4-cyanophenyl 4‟-n-octyloxy-2-fluorobenzoate), just behind the collapse point in the -A isotherm a 'spike', i.e. a rapid fall of the surface pressure appears and a large hysteresis of expansion and compression isotherms is observed, indicating on the instability of the monolayers. This leads to the conclusion that the molecular structure of the rigid core of calamitic liquid crystals strongly influences the stability of the monolayer at the air-water interface. The difference in the -A isotherm shapes for two fluoro-compounds points out that the monolayer stability can be also affected by the position of the lateral group. The steepness of the isotherm reflects the monolayer rigidity. It is seen that it is dependent on the molecular structure of the liquid crystal too. Figures 4 and 5 show isotherms for some members of 4-n-alkyloxy-4‟-cyanobiphenyl (nOCB) and trans-4-n-alkyl(4‟-cyanophenyl)-hexane (nPCH) series. It is seen that the values of the area and the pressure at the collapse point as well as the isotherm steepness are dependent also on the hydrocarbon chain length in the molecule. The values of the collapse areas found from the isotherms suggest that in the monolayer formed of all the compounds investigated the rigid cores of the molecules must be tilted with respect to the water surface (Fig. 6).
Figure 4. Surface pressure-area isotherms of Langmuir films formed of members of nOCB series [24].
Further information about a polar molecules organization, particularly at early stages of the film compression when the surface pressure is still zero, gives the surface potential measurement. For all the liquid crystals under investigation the dependence of the surface potential, V, on the average area, A, were recorded and Figs. 7-10 present representative
60
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
examples of V-A isotherm (solid curve), recorded simultaneously with the -A isotherm (dotted curve curve), as well as the dipole moment-area (-A) isotherm (dashed curve), calculated on the basis of Eq. (1), for the liquid crystals 7PCH, 7OCB, 6CPB, and 8OCFPB. In Tables 1-5 the features of -A and V-A isotherms of the monolayers of all the liquid crystals which were able to form the compressible Langmuir film are gathered. A 0π and A ΔV 0 are the values of the area at which, respectively, and V start to increase, whereas AC, C, and VC are the values of, respectively, the area, the surface pressure, and the surface potential at the collapse point. On the basis of AC the average tilt angle between the normal to the water surface and the long molecular axis (Fig. 6) were calculated by assuming that the mean molecular area is determined only by the rigid core of the liquid crystal molecule. The values of the angle as well as of , calculated at the collapse pressure, are also given in Tables 3-7.
Figure 5. Surface-pressure-area isotherms of Langmuir films formed of members of nPCH series [23].
Figure 6. Definition of the angle between the normal to the water surface and the long molecular axis (when instead of water the surface is quartz slide, this angle is marked as ) [24].
Molecular Organization of Thermotropic Liquid Crystals …
61
Table 3. Features of -A and V-A isotherms, the average angle between the long molecular axis and the normal to the water surface, , and the effective dipole moment, , of members of homologous series of nCB in Langmuir films. π
Compound A 0 /nm2 AC/nm2 πC/mNm-1 φ/deg 4CB 5CB 6CB 7CB 8CB 9CB 10CB 11CB 12CB
0.29 0.39 0.45 0.46 0.47 0.46 0.51 0.47 0.49
0.20 0.30 0.36 0.37 0.41 0.40 0.44 0.40 0.43
4.3 4.8 5.3 5.0 4.8 4.6 4.4 4.6 4.6
25 39 49 51 60 57 68 57 65
2 A ΔV 0 /nm ΔVC/V
0.41 0.60 0.57 0.56 0.65 0.54 0.58 0.64 0.72
0.590 0.610 0.618 0.663 0.630 0.619 0.683 0.744 0.787
μ/D 0.31 0.48 0.58 0.65 0.67 0.65 0.79 0.94 0.90
Table 4. Features of -A and V-A isotherms, the average angle between the long molecular axis and the normal to the water surface, , and the effective dipole moment, , of members of homologous series of nPCH in Langmuir films. Compound
A 0π /nm2
AC/nm2
πC/mNm-1
φ/deg
2 A ΔV 0 /nm
ΔVC/V
μ/D
4PCH 5PCH 6PCH 7PCH 8PCH 9PCH 10PCH
0.61 0.59 0.58 0.61 0.57 0.54 0.53
0.42 0.45 0.45 0.47 0.48 0.47 0.47
6.0 5.4 5.3 4.8 5.3 4.6 3.5
45 50 50 53 54 53 53
0.95 0.90 0.65 0.86 0.71 0.73 0.72
0.502 0.534 0.551 0.544 0.520 0.589 0.649
0.56 0.64 0.67 0.68 0.73 0.73 0.81
The shapes of V-A and -A isotherms for all the liquid crystals investigated are quite similar, although the values of V and at the characteristic points of the isotherms are different for various liquid crystals. In all the cases the rise of V is observed earlier than the rise of . V first increases rather sharply up to the area which coincides with the onset area for . Next, V keeps on growing but at a slower rate and reaches the maximum at the collapse point. Behind this point V remains constant. As the measured value of V is contributed only by the first monolayer coming into contact with the water [27], this suggests that the dipole density in this layer does not change during reduction of the area. Thus, during the compression, the molecules do not assume more and more vertical alignment, but are ‟pushed out‟ above the first monolayer being in the contact with the water and align on its top in more or less ordered way. Therefore, the dipole moment, , calculated directly from Eq. (1) has a physical meaning only up to the collapse point and is not shown behind this point in Figs. 7-10.
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
62
Table 5. Features of -A and V-A isotherms, the average angle between the long molecular axis and the normal to the water surface, , and the effective dipole moment, , of members of homologous series of nOCB for Langmuir films. π
Compound A 0 /nm2 AC/nm2 πC/mNm-1 φ/deg 5OCB 6OCB 7OCB 8OCB 9OCB
0.34 0.45 0.45 0.44 0.38
0.22 0.32 0.36 0.40 0.33
5.8 5.8 5.8 3.6 1.9
24 36 41 47 37
2 A ΔV 0 /nm ΔVC/V
0.44 0.61 0.62 0.57 -a
0.611 0.643 0.683 0.675 -a
μ/D 0.40 0.54 0.69 0.70 -a
a
- ΔV-A isotherm impossible to record
Table 6. Features of -A and V-A isotherms, the average angle between the long molecular axis and the normal to the water surface, , and the effective dipole moment, , of members of homologous series of nCPB in Langmuir films. π
Compound A 0 /nm2 AC/nm2 πC/mNm-1 φ/deg 6CPB 7CPB 8CPB 9CPB
0.67 0.62 0.62 0.57
0.42 0.42 0.40 0.41
7.0 7.2 6.2 7.8
46 46 43 45
2 A ΔV 0 /nm ΔVC/V
0.88 0.77 0.85 0.83
0.624 0.624 0.710 0.740
μ/D 0.75 0.75 0.87 0.81
Table 7. Features of -A and V-A isotherms, the average angle between the long molecular axis and the normal to the water surface, , and the effective dipole moment, , of 8OCFPB and 8OCPFB in Langmuir films. π
Compound A 0 /nm2 AC/nm2 πC/mNm-1 φ/deg 8OCFPB 8OCPFB
0.72 0.76
0.45 0.45
7.4 8.3
40 40
2 A ΔV 0 /nm ΔVC/V
0.91 1.02
0.551 0.577
μ/D 0.67 0.73
The quantity is the so-called apparent or effective dipole moment and cannot be mistaken for the dipole moment of an isolated molecule, because it is influenced by several factors, first of all by various dipole fields. According, e.g. to the Demchak-Fort model [28], is composed of three independent contributions arising from (i) orientation of water dipoles in the vicinity of the headgroup, (ii) the headgroup dipoles, and (iii) the hydrophobic part dipoles. Further, in our calculations we assumed, as it is made customary [27,29], that r = 1, although it is known that dipoles in a monolayer may be embedded in media with distinct dielectric constant values (r > 1), which depends on whether these dipoles are at the monolayer-water or monolayer-air interface [30,31]. For the liquid crystals under investigation rises together with the rise of V up to the highest value being reached at the area corresponding to the onset for the surface pressure. Such a value of remains almost constant up to the collapse point (the product VA is constant in the region between vertical lines in Figs. 7-10). The runs of -A isotherms
Molecular Organization of Thermotropic Liquid Crystals …
63
indicate that at a large area available for the liquid crystal molecules, they lie almost horizontally at the water surface. Upon compression, the molecules start to interact and at some critical area the hydrophobic parts of them lift up from the water surface causing their tilted alignment with respect to the horizontal direction. Such changes of the orientation are confirmed by the significant increase of V and at this stage. Since reaches the maximal value at the area corresponding to the surface pressure onset and then remains constant (or almost constant), we suppose that the tilt angle of the mesogenic molecules at the air-water interface is settled already at the beginning of the formation of the condensed monolayer.
Figure 7. Surface potential, V (solid curve), surface pressure, (dotted curve) and effective dipole moment, (dashed curve) as a function of the mean molecular area, A for Langmuir film of 7PCH [24]. The scale in ordinate axis for V and is the same.
Figure 8. Surface potential, V (solid curve), surface pressure, (dotted curve) and effective dipole moment, (dashed curve) as a function of the mean molecular area, A for Langmuir film of 7OCB [24]. The scale in ordinate axis for V and is the same.
64
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
Figure 9. Surface potential, V (solid curve), surface pressure, (dotted curve) and effective dipole moment, (dashed curve) as a function of the mean molecular area, A for Langmuir film of 6CPB [24]. The scale in ordinate axis for V and is the same.
Figure 10. Surface potential, V (solid curve), surface pressure, (dotted curve) and effective dipole moment, (dashed curve) as a function of the mean molecular area, A for Langmuir film of 8OCFPB [24]. The scale in ordinate axis for V and is the same.
Molecular Organization of Thermotropic Liquid Crystals …
(a)
(b)
(c)
(d)
65
Figure 11. BAM images of 8CB Langmuir film at mean molecular areas A = 0.55 nm2 (a), 0.44 (b), 0.26 (c) and 0.09 nm2 (b). The area of images is 0.35 x 0.30 mm2.
The direct observation of the morphology of Langmuir films enables Brewster angle microscopy. BAM images of the liquid crystal 8CB recorded by us were similar to those known from the literature [6,7]. In the region of coexistence of the gas and liquid phases (region I – Fig. 2) we observed condensed monolayer islands in equilibrium with a foam-like structure (Fig. 11a). As the surface pressure raised (region II), the islands joined together into a completely packed monolayer, giving a homogeneous picture (Fig. 11b). Just after the collapse point in the first plateau region (III), small brighter circular or oval domains were observed, and these grew with reduction of the film area (Fig. 11c). By further reduction of the available area, when the domains observed became sufficiently large, they deformed and coalesced. The domains of 8CB in the plateau region appeared to be of homogeneous reflectivity, meaning that they have equal thickness. At the second rise of (region IV), a homogeneous multilayer structure (trilayer: monolayer covered by bilayer) was created, and in the second plateau region (V), new domains were formed (Fig. 11d). These domains are significantly brighter than those in region III, thus they indicate the creation of the next uniform layer.
66
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
(a)
(b)
Figure 12. BAM images of 5CB in Langmuir film at A = 0.25 (a) and 0.10 (b). The area of images is 0.35x0.30 mm2.
Similar BAM images as for 8CB were obtained for 9CB and 10CB, i.e. for these liquid crystals which have the smectic A (SmA) phase in the bulk and are able to create a stable Langmuir film. However, BAM images of the liquid crystals having only the nematic (N) phase were similar to those of 8CB only up to the collapse point. By the compression beyond this point we observed the appearance of the domains of much higher brightness surrounded by interference rings. Fig. 12 presents, as an example, BAM images of the Langmuir film formed from 5CB at two different areas in the plateau region of the surface pressure. It is seen that with the decrease of the A value the number of the domains rises. However, they are not in collision and do not join together. The higher brightness of the domains in comparison with those observed for 8CB-10CB in this region indicates that they have higher thickness. Similar BAM images behind the collapse point as for 5CB were obtained for all the nematogens giving stable monolayers (4CB, 5CB, 5OCB, 6OCB, 4PCH-8PCH, 6CPB, 7CPB, 8OCFPB). For 7CB and 7OCB, which are precursors of the smectogenic compounds in the homologous series, the domains with the interference rings appeared at the end of the plateau region [14,23,24]. The detailed analysis of the rings structure suggests that the domains grow in the third dimension when A decreases. This leads to the conclusion that we have to deal here with 3D objects. Our observations seem to suggest that the shape and character of the domains observed beyond the collapse point can be related to the mesophase which the compounds possess in the bulk. This suggestion could be confirmed by BAM images of 8CB in the Langmuir film recorded at different temperatures in the whole mesophase region, i.e. both in SmA and N phases. Previously, Suresh and Bhattacharyya [32] investigated the 8CB monolayer on the water surface at different temperatures by means of a fluorescence microscope. At temperatures corresponding to the existence of SmA phase in the bulk they observed optically flat domains representing “trilayer” phase (first plateau region of -A isotherm) or regular “multilayer” phase (second plateau region). With an increase of temperature above the SmA-N transition, instead of the multilayer domains, the lens-shaped 3D domains came into existence. Similar domains were observed also at temperatures corresponding to the isotropic phase in the bulk.
Molecular Organization of Thermotropic Liquid Crystals …
67
Figure 13. Surface pressure-area isotherms of 8CB in Langmuir film at T = 26oC (SmA phase), 40oC (N phase), and 45oC (isotropic phase). Marks indicate the area values at which BAM images presented in Fig. 14 were recorded.
Our BAM studies revealed similar results. Figs. 13 and 14 illustrates how -A isotherms and BAM images obtained at A 0.2 nm2 change when the temperature rises (when the available area is greater than 0.2 nm2, the run of the isotherm and BAM images recorded at temperatures corresponding to SmA and N phases do not change and resemble those obtained at 21oC and presented in Fig. 11). At T = 26oC (SmA phase) the second plateau on the isotherm is still observed (Fig. 13a) and flat domains are seen to the end of the compression
68
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
process (Fig. 14b), although they have now smaller sizes than at lower T. The second plateau disappears in the N phase (Fig. 13b) and the domains with the interference rings appear, but not before A < 0.1 nm2 (Fig. 14d). At the temperatures corresponding to the isotropic phase (Fig. 13c) the 3D objects are seen earlier, already at A 0.25 nm2 (Fig. 14e). Thus, following Suresh and Bhattacharyya [32] we can postulate that the domains found for 8CB monolayer for A less than 0.2 nm2 exhibit different phases depending on temperature. At temperatures below the SmA-N transition in the bulk they are flat and contain molecules aligned in an interdigitated bilayer, like in SmA phase. Next they become lens-shaped with a nematic order, and at higher temperatures the domains may contain molecules with random (isotropic) arrangement.
(a)
b) T = 26ºC (SmA)
(c)
d) T = 40ºC (N)
(e)
(f) T = 45ºC (Iso)
Figure 14. BAM images of 8CB in Langmuir film at A = 0.16 (a,c), 0.09 (b,d,f), and 0.26 (e) nm 2. The area of images is 0.35x0.30 mm2.
Molecular Organization of Thermotropic Liquid Crystals …
69
On the basis of our BAM studies we can conclude that there exists some correlation between the molecular organization of liquid crystals at the air-water interface and their ability to create the appropriate phase in the bulk. Whereas for smectogenic molecules only optically flat domains have been found, the Langmuir films formed of nematogenic molecules have been characterized by existence of 3D lens-shaped domains just beyond the collapse point or at the end of the plateau region. When the liquid crystal has both SmA and N phases the type of the domains depends strongly on the temperature. The proposed organization of liquid crystal molecules in the flat and droplet-like domains is illustrated in Fig. 15. As for nematogenic liquid crystals the constant value of V beyond the collapse point is also observed this leads to the conclusion that in 3D domains created on the top of the homogeneous monolayer mostly antiparallel alignment of molecules occur, similarly as it takes place in the flat domains.
Figure 15. Schematic representation of molecular organization in flat (a) and lens-like (b) domains [23].
3.1.2. Electronic Absorption Spectra of Langmuir-Blodgett Films Figure 16 shows the absorption spectra of the LB films of the liquid crystals recorded in UV region from 225 nm to 350 nm, whereas in Table 8 the position of the absorption maximum, max, and the half-bandwidth of the absorption band, , for the representative liquid crystals with n = 8 as the LB films are presented. The absorption maximum of the liquid crystals from nPCH series appears outside the spectral region used in the experiment (< 225 nm). It follows from the data presented here that both the absorption band position as well as the band width strongly depend on the molecular structure of the liquid crystals. For comparison, Table 8 gathers the values of max and for the liquid crystals dissolved in chloroform. The data given in Table 8 indicate that the wavelengths of the absorption band maximum of liquid crystals in the LB film are almost the same as in the diluted solution. However, the half-bandwidths in the LB film are significantly larger than those in chloroform. As in the chloroform the measurements were made at very low liquid crystal concentration, it is clear that the absorption spectra obtained are characteristic for monomers. Thus, the significant broadening of the spectra of the LB films could be attributed to the creation of some kinds of
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
70
aggregates between liquid crystal molecules, although the influence of the surface interaction cannot be excluded.
Figure 16. Absorption spectra of Langmuir film of representative liquid crystals with n = 8 [24].
Table 8. The position of the absorption maximum, max, and the half-bandwidth of the absorption band, , for liquid crystals with n = 8 dissolved in LB film and in chloroform at XM = 1.710-7.
Compound 8CB 8OCB 8CPB 8OCFPB 8OCPFB
LB film Chloroform λmax/nm δ/cm-1 λmax/nm δ/cm-1 -1 Δλmax = ±1nm Δδ = ±50 cm Δλmax = ±1nm Δδ = ±10 cm-1 281 5700 283 5180 295 6250 298 5650 249 7250 251 5000 276 5450 277 5010 264 6600 263 5900
In order to evaluate quantitatively the orientation of the liquid crystal molecules in the LB films, polarized absorption spectra were recorded and the linear dichroism (LD) was determined. We defined LD as follows [33]:
LD
AP AS , AP AS
(2)
where AP and AS are the absorbance values at the band maximum for the light polarized parallel and perpendicularly to the plane of incidence, respectively.
Molecular Organization of Thermotropic Liquid Crystals …
71
LD can be related to the angle of incidence, (Fig. 1) in the following way:
LD
2 tan 2 , 1 cos 2 2 2 tan sin 2
(3)
where is the angle between the absorption transition dipole moment vector and the normal to the plane of the LB film. Figure 17a shows the polarized absorption spectra recorded at = 0° for 7OCB in the LB film, as an example. It can be seen that, for this liquid crystal, the value of the linear dichroism for the light incident perpendicularly to the quartz surface, LD=0, is zero. This means that the movement of the quartz slide during deposition did not disturb the homogeneity of the molecular alignment. Thus, the angle can be calculated from Eq. (3) on the basis of the spectra measured at the angle ≠ 0o. The spectra of polarized absorption components recorded at = 60o for 7OCB are presented in Fig. 14b.
Figure 17. Absorption spectra of the light polarized parallel (Ap) and perpendicularly (As) to the incidence plane for 7OCB as LB film. The incidence angle was 0o (a) and 60o (b) [24].
On the basis of the angle it is possible to obtain information about the orientation of the liquid crystals molecules with respect to the normal to the solid substrate surface. It is, however, necessary to know the angle between the absorption transition moment and the long axis of the liquid crystal molecule. To a first approximation, we can assume that for the liquid crystals under investigation this angle is equal to zero. Thus, the angles reflect directly the orientation of the mesogenic molecules in the LB films and for the liquid crystals with n = 8 they are collected in Table 9. It is seen that for all the liquid crystals the angle has similar value, equal to about 60o. This means that the liquid crystal molecules are significantly tilted towards the quartz slide surface, like to the water surface in the Langmuir films. Comparing
72
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
the values of and (Tables 3-7) it is seen that the rigid cores of the rod-shaped liquid crystal molecules are significantly more tilted toward the solid surface in the LB films than toward the water in the Langmuir films. This indicates that during the transfer of the monolayer from the air-water interface onto the quartz slide a molecular rearrangement can take place. However, one should keep in the mind that the different tilt of molecules with respect to the surface can be also, at least partially, due to the surface interactions of the liquid crystal molecules with the solid substrate which are different than with the water. Table 9. Average angle between the rigid molecular core and the normal to the quartz surface, , for liquid crystals with n = 8. Compound 8CB 8OCB 8CPB 8OCFPB 8OCPFB
β/deg 65 60 59 62 60
3.2. Langmuir and Langmuir-Blodgett Films of Azo Dye/Liquid Crystal Mixtures 3.2.1. Langmuir Film Characterization The azo dyes dissolved in chloroform were spread on the water surface in the Langmuir through and the monolayer compression test was performed. We found, however, that the monolayer cannot be compressed: the surface pressure remained continuously at zero and the bulk phase was observed to form. This means that none of the azo dyes under investigation can produce stable and compressible monolayer, although all they possess terminal and/or lateral polar group in the molecular structure. Therefore, in order to study the dye properties in Langmuir and LB films it was necessary to use the supporting matrix. The azo dyes were mixed with two chosen liquid crystals, namely 8CB and 8PCH, at various concentrations. It was ascertained that up to the dye molar fraction XM = 0.5 (sometimes up to 0.6), the compression of the monolayer formed of dye/liquid crystal mixture was possible and stable Langmuir films were obtained. Figures 18 and 19 present -A isotherms of the Langmuir films of the liquid crystals and of 1/8CB and 3/8PCH mixtures, as examples, whereas the characteristic values of -A isotherms for monolayers of all azo dyes mixed with the liquid crystal (dyes 5-9 were mixed only with 8CB) at XM = 0.1, 0.3 and 0.5 are resumed in Tables 10 and 11. The isotherms were recorded both during compression and expansion processes and only small differences in the isotherm runs were found. From the course of the -A isotherms for all the dye/liquid crystal mixtures it follows that the rise of begins at smaller and smaller values as XM of the dye increases. This indicates that the presence of the dye improves the packing of molecules in the Langmuir film. As a result the tilt angle decreases as compared with the tilt angle of 8CB and 8PCH molecules (see: Tables 3 and 4). Knowing the area of the dye molecule and taking into account the mixture composition we were able to estimate the average angles, av, for mixed monolayers. They are gathered in Tables 10 and 11, too. One should keep, however, in
Molecular Organization of Thermotropic Liquid Crystals …
73
the mind that such estimation is very rough, because in general the splay deformation of the Langmuir film can occur.
Figure 18. Surface pressure-mean molecular area isotherms of Langmuir films of pure 8CB (1) and of binary mixtures of dye 1 in 8CB with XM of 0.1 (2), 0.2 (3), 0.3 (4), 0.4 (5), and 0.5 (6).
Figure 19. Surface pressure-mean molecular area isotherms of Langmuir films of pure 8PCH (1) and of binary mixtures of dye 3 in 8PCH with XM of 0.1 (2), 0.2 (3), 0.3 (4), 0.4 (5), 0.5 (6), and 0.6 (7) [13].
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
74
The increase of the dye content in the mixture causes the better rigidity and stability of the Langmuir film, as is confirmed by the rise of the isotherm steepness and the value of C. For the most mixtures the characteristic dye concentration is XM = 0.3 or 0.4. At such content of the dye, both the tilt angle of the -A plot (with respect to the horizontal direction) and C have the highest values. Table 10. Features of -A and V-A isotherms, the average angle between the long molecular axis and the normal to the water surface, av, and the effective dipole moment, , of azo dye/8CB mixtures in Langmuir films. Nup/Ndown is the ratio of molecules with dipole moment pointing in opposite directions in the monolayer.
Compound XM
A0
0.1 0.3 0.5 0.1 0.3 0.5
/nm2 0.48 0.38 0.24 0.18 0.36 0.31 0.30
3/8CB
0.1 0.3 0.5
4/8CB
0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5
8CB 1/8CB 2/8CB
5/8CB 6/8CB 7/8CB 8/8CB 9/8CB
AC C av /nm2 /mN·m-1 /deg
A0V
VC /V
Nup/Ndown /D
0.41 0.29 0.20 0.14 0.30 0.27 0.28
4.8 6.1 19.0 15.7 7.2 13.0 12.4
61 37 23 15 38 31 30
/nm2 0.65 0.54 0.46 0.35 0.52 0.55 0.50
0.38 0.25 0.24
0.31 0.17 0.20
6.0 21.0 19.0
39 18 20
0.50 0.51 0.46
0.584 0.48 0.341 0.15 0.251 0.13
0.15 0.39 0.40
0.41 0.34 0.24 0.42 0.32 0.26 0.46 0.30 0.25 0.43 0.27 0.20 0.47 0.39 0.27 0.44 0.37 0.27
0.35 0.27 0.20 0.32 0.24 0.20 0.37 0.24 0.20 0.29 0.20 0.14 0.37 0.30 0.20 0.37 0.31 0.23
6.5 6.5 5.9 5.4 7.0 4.0 5.2 7.0 9.0 6.7 11.6 6.7 4.9 5.1 4.2 4.6 4.3 4.1
39 29 18 31 15 11 35 15 10 33 19 11 45 30 17 45 31 19
0.60 0.65 0.43 0.65 0.70 0.67 0.60 0.45 0.50 0.52 0.50 0.37 0.60 0.47 0.44 0.53 0.45 0.38
0.595 0.580 0.568 0.618 0.524 0.352 0.624 0.461 0.388 0.607 0.411 0.465 0.640 0.671 0.627 0.636 0.638 0.600
0.10 0.19 0.28 0.07 0.22 0.34 0.07 0.30 0.34 0.13 0.31 0.34 0.01 0.10 0.22 0.05 0.12 0.24
0.630 0.626 0.415 0.395 0.611 0.422 0.319
0.67 0.48 0.22 0.15 0.49 0.30 0.24
0.15 0.34 0.39 0.14 0.28 0.32
0.55 0.42 0.30 0.61 0.40 0.23 0.61 0.29 0.23 0.52 0.27 0.23 0.70 0.57 0.40 0.64 0.54 0.37
This observation points out that the azo dye molecules are able to „stiffen‟ the molecules of liquid crystals. As the XM of the dye increases further, C value decreases indicating that the monolayer stability grows smaller. This means that for XM 0.4, the liquid crystal cannot play further the role of a host. Although the compression is still possible, in the most cases the average area per molecule is too small for even the most dense packing of molecules in a
Molecular Organization of Thermotropic Liquid Crystals …
75
monolayer, which suggests the creation of 3D domains. Comparing the results gathered in Table 10 with those in Table 11 it is seen that all the effects mentioned above depend in some extent on the kind of the liquid crystal. The influence of the molecular structure of the dyes on the behavior of the azo dye/liquid crystal mixtures in the Langmuir film is also distinctly seen. Table 11. Features of -A and V-A isotherms, the average angle between the long molecular axis and the normal to the water surface, av, and the effective dipole moment, , of azo dye/8PCH mixtures in Langmuir films. Nup/Ndown is the ratio of molecules with dipole moment pointing in opposite directions in the monolayer.
Compound XM 8PCH 1/8PCH 2/8PCH 3/8PCH
4/8PCH
0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5
A0 2
/nm 0.58 0.54 0.35 0.23 0.58 0.41 0.30 0.54 0.46 0.36 0.51 0.47 0.32
AC /nm2 48 0.45 0.23 0.17 0.49 0.32 0.25 0.45 0.34 0.27 0.43 0.40 0.26
C av /mN·m-1 /deg 5.3 6.3 16.0 15.7 6.4 7.9 11.5 6.6 6.0 5.2 5.8 5.9 5.9
54 51 23 17 42 32 24 49 33 27 46 39 24
A0V 2
/nm 0.72 0.70 0.63 0.44 0.73 0.61 0.49 0.66 0.60 0.52 0.64 0.65 0.48
VC /V 0.520 0.491 0.379 0.298 0.470 0.329 0.270 0.492 0.431 0.364 0.528 0.513 0.511
Nup/Ndown /D 0.64 0.57 0.23 0.13 0.59 0.28 0.18 0.59 0.39 0.26 0.60 0.55 0.35
0.05 0.33 0.40 0.04 0.28 0.36 0.04 0.20 0.30 0.03 0.07 0.23
The changes of the isotherm run with the Langmuir film composition for the azo dye/liquid crystal mixtures indicate on the interactions between two components molecules. The kind of these interactions can be followed in Figs. 20-22, in which the excess of the average area per molecule, AE as a function of XM for the dye/liquid crystal mixtures in the Langmuir films is presented. The excess area is defined as follows:
AE A12 ( X M 1 A1 X M 2 A2 ).
(4)
A12 is here the average molecular area in the two-component film, XM1 and XM2 are the molar fractions of the components, and A1 and A2 are the single component areas taken at the same as A12. In our experiment the values of A were taken at = 3 mN/m for dyes 1-4 and 4 mN/m for dyes 5-9. If AE is equal to zero, the average area per molecule follows the additivity rule, which means that in the mixture ideal mixing or complete immiscibility occurs. Deviation from zero, either positive or negative, indicates miscibility and non-ideal behavior. In Figs. 20-22 the noticeable deviation from the additivity rule is observed. For dyes 1 mixed with both liquid crystals and dyes 5, 6 and 7 mixed with 8CB this deviation is predominantly negative meaning a contraction of the two-component films due to attractive interactions among dye and liquid crystal molecules [8,34]. In the case of dyes 2, 3 and 4 the deviation is mostly
76
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
negative for their mixtures with 8CB, and positive when they are mixed with 8PCH. This indicates that the cyclohexane ring present in the 8PCH molecule can cause repulsive interactions. The positive values of AE occur here also for 8/8CB and 9/8CB mixtures, indicating on repulsive intermolecular interactions [8,34]. The values of AE 0 for all the binary mixtures investigated would suggest that two components in the Langmuir films are always good miscible. However, the information from the surface phase rule [8] should be taken into account additionally. This rule states that if the components are miscible, the C value should change with the mixture composition. Meanwhile, from the dependence of the C value on the composition of the Langmuir films of the dye/liquid crystal mixtures (Table 10 and 11) follows that in the case of dyes 4, 8 and 9 mixed with 8CB and 3 and 4 mixed with 8PCH the immiscibility or at least only partial miscibility of two components can be postulated. This results from the fact that although the additivity rule is not fulfilled, C remains constant.
Figure 20. Plot of the excess of the mean molecular area per molecule, AE of dyes 1-4 mixed with 8CB versus XM of dyes at = 3 mN/m: 1 (1), 2 (2), 3 (3), and 4 (4).
Figure 21. Plot of the excess of the mean molecular area per molecule, A E of dyes 5-9 mixed with 8CB versus XM of a dye at = 4 mN/m: 5 (1), 6 (2), 7 (3), 8 (4), and 9 (5) [17].
Molecular Organization of Thermotropic Liquid Crystals …
77
Figure 22. Plot of the excess of the mean molecular area per molecule, AE of dyes 1-4 mixed with 8PCH versus XM of dyes at = 3 mN/m: 1 (1), 2 (2), 3 (3), and 4 (4).
For the Langmuir films of all the azo dye/liquid crystals mixtures under investigation the dependence of the surface potential, V, on the average area, A, were recorded and Fig. 23 illustrates the V-A isotherm (solid curve), recorded with the -A isotherm (dotted curve), and the dipole moment-area (-A) isotherm (dashed curve), calculated from Eq. (1), for 8CB and 2/8CB mixtures at various XM, as examples. In Tables 10 and 11 the features of V-A isotherms of the monolayers of all the mixtures are listed.
16
0.3
8 6
0.3
0.4
A/nm
2
0.5
0.6
-1
/mNm
20 18
12
0.4
10 0.3
8 6
0.2
4
0.1
2
0.0
0 0.5 2
0.3
0.4
0.5
0.6
0.7
0.6
0.7
0.7
d)
0.6
16
0.5
14
0.4
0.0 0.2
2
0.6
16
A/nm
0.1
A/nm
c)
0.3
0.2
0 0.1
0.7 0.7
0.2
0.3
8
0.5
14 12
0.4
10 0.3
8 6
0.2
4
0.1
2
0.0
0 0.1
V/V; /D
0.2
0.4
10
2
-1
0.1
0.5
12
4
0.0
0
14
6
0.1
2
0.1
-1
0.2
4
18
/mNm
0.4
10
0.6
16
/mNm
-1
/mNm
12
0.7
b)
18
0.5
14
20
20
0.6
V/V; /D
0.7
a)
V/V; /D
18
V/V; /D
20
0.2
0.3
0.4
A/nm
0.5
0.6
0.7
2
Figure 23. Surface potential, V (solid curve), surface pressure, (dotted curve), and effective dipole moment, (dashed curve) as a function of the mean molecular area, A for Langmuir film of 8CB (a) and 2/8CB mixtures at XM equal to 0.1 (b), 0.3 (c) and 0.5 (d) [15].
78
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
From the data presented in Fig. 23 and in Tables 10 and 11 follows that with the increase of the dye content in the mixture, although C values rises or remains constant, VC decreases. As a result, for the dye/liquid crystal mixtures is always smaller than that for the liquid crystal itself and decreases as the XM of the dye rises. This is rather unexpected result taking into account the fact that the molecules in the Langmuir films formed of the mixtures align more and more perpendicularly to the water surface with the increase of the dye content (see values in Table 8 and 9) – in this case should be higher and higher. Thus, we need to assume that the dye dipoles are aligned mostly opposite to the dipoles of the liquid crystal molecules leading to the diminishing of the total effective dipole moment. The dipole moments of the liquid crystal molecules in the first monolayer at the air-water interface are directed towards the water (down) giving the effective dipole moment . Let us now estimate the number of the molecules in the dye/liquid crystal mixtures with the dipole moments aligned in the opposite direction (up). Assuming that in the monolayer at the water surface there exists Nup and Ndown molecules, the effective dipole moment ' is obtained, which is smaller than . This decrease of is due to the compensation of the resultant dipole moment by pairs of molecules, in which the dipole moments are antiparallel arranged. As the dipole moments of the polar groups –CN and –NO2 are similar ( 4 D), we assume for simplicity that values of the dye and liquid crystal molecules are the same. Then the ratio of Nup/Ndown can be calculated from the relation:
( N down 2 N up ) / N down ' / .
(5)
The results for various XM of the dyes mixed with 8CB or 8PCH are presented in Tables 10 and 11. Comparison of the data for given dye in two liquid crystals indicate on the different arrangement of the dye molecules in the mixtures with 8CB and 8PCH at low concentration. In the mixtures with 8PCH only some part of the dye molecules align with the dipole moment directed from the water to the air. For the mixtures of some dyes (1, 2, 3, 7) with 8CB it is necessary to assume that not only the dye molecules but also some liquid crystal molecules are directed "up". When XM rises, the fraction of Nup molecules in the mixtures with both liquid crystals becomes similar and at MF > 0.3 it is smaller than the whole number of the dye molecules. However, the alignment of the dye molecules with the dipole moment directed towards the air is further strongly preferred. We looked for the correlation between the value and the direction of the dipole moment of the given dye molecule and the diminishing of values of the monolayer after the dye addition. Dyes 1, 2, 4, 5, 7 and 8 have similar value of the dipole moment, with different directions of it. The value of the dipole moment of dyes 3, 6 and 9 is smaller because here the –NO2 group ( 4 D) is replaced by –Cl group ( 1.5 D). However, the values of calculated from Eq. (1) are not associated with these facts. Meanwhile, the smallest changes of V and appear for the Langmuir films of 4/8CB, 8/8CB, 9/8CB, 3/8PCH and 4/8PCH mixtures. As in these mixtures the immiscibility or at least partial miscibility of the dye and liquid crystal molecules is observed, it is reasonable to assume that in such a case, the dye molecules form domains in which the dipolar groups of molecules are directed mostly “down” as a result of attractive interactions with the water (the dye molecules have no distinct hydrophobic part). Thus, the dipole-dipole interaction between both kinds of molecules is
Molecular Organization of Thermotropic Liquid Crystals …
79
hindered making the creation of the antiparallel pairs consisted of the dye and liquid crystal molecules more difficult, which is confirmed by the small value of the ratio of Nup/Ndown for these mixtures. Moreover, V does not change significantly and the presence of the dye does not improve the stability of the Langmuir film (C remains constant). This is illustrated schematically in Fig. 24a. However, in the case of good miscibility, individual dye molecules can point the dipole moment towards air and form antiparallel aligned dimers with liquid crystal molecules (Fig. 24b).
Figure 24. Schematic representation of microscopic polar ordering in Langmuir film of dye/liquid crystal mixture before the collapse point in the case of immiscibility or partial miscibility (a) and good miscibility (b) of both components. Filled and open arrows represent dipole moments of molecules of liquid crystal and dye, respectively [15].
The runs of V behind the collapse point indicate that this value is either constant or drops slightly upon reduction of the available area. The decreasing of V is not bigger than 20% and is observed only to XM = 0.3 (Figs. 23b and 23c). At XM > 0.3, V stays constant, which is seen in Fig. 23d. This means that in the interdigitated bilayers (dye/8CB mixtures) or 3D domains (dye/8PCH mixtures) created on the top of the first monolayer coming into the contact with the water, the antiparallel arrangement of the dye and liquid crystal molecules dominates (Fig. 25) causing that V does not change significantly. The diminishing of V, observed for some mixtures, could solely suggest the very small excess of the molecules directed with the dipole moment towards the air. In order to obtain further information about organization of azo dye and liquid crystal molecules in the two-component monolayer at the air-water interface, the BAM images were recorded at various stages of the Langmuir film creation. In Figs. 26a and 27a are shown -A isotherms for Langmuir films of 8CB mixed with dyes 1 and 4, respectively, at XM = 0.1 with marks of the compression stages at which BAM images, presented in Figs. 26b and 27b, were recorded. There were almost no differences between the structures of pure 8CB film and those of 1/8CB film. Before the surface potential and the surface pressure start to rise (1), we observed brighter islands of molecules on the dark water surface. These islands come together to form a homogeneous film when the surface pressure is still zero but the surface potential starts to rise. Further compression makes the film completely homogeneous (2). After the collapse point small domains appear (3),
80
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
which grow continuously as the monolayer is further compressed. The surface pressure increases in this region (unlike to the case of the Langmuir film of 8CB), indicating the presence of the dye molecules in the monolayer, which, however, do not perturb the alignment of 8CB molecules and the liquid crystal domains can join together as the available area is limited (4). The images of the mixtures of dyes 2, 3, 5, 6 and 7 with 8CB are similar to those of 1/8CB. The behaviour of 4/8CB film is different. Already at = 0 (1) in the foamlike structure bright shimmer areas with irregular boundaries are seen, which exist also beyond the collapse point (2). The creation of the oval domains is also seen (3,4), but they do not pack together, solely their brightness increases. As the similar BAM images for dyes 8 and 9 mixed with 8CB were obtained, we suppose that this effect is connected with the immiscibility of two components in the Langmuir film. For dyes 3 and 4 mixed with 8PCH also the phase separation was observed and it was reflected in BAM images too (data not shown). However, for the Langmuir film of 1/8PCH and 2/8PCH at XM = 0.1 we obtained very similar images as for pure 8PCH [14,23]. They are shown for 2/8PCH in Fig. 28, together with -A isotherm. The objects with interference rings are seen very distinctly. The number of these objects rises when the available area on the water surface decreases.
Figure 25. Schematic representation of microscopic polar ordering in Langmuir film of dye/8CB (a) and dye/8PCH (b) mixtures beyond the collapse point. Filled and open arrows represent dipole moments of molecules of liquid crystal and dye, respectively [15].
Molecular Organization of Thermotropic Liquid Crystals …
(1)
(2)
(3)
(4)
81
Figure 26. Surface pressure-mean molecular area isotherms of 1/8CB mixture (XM = 0.1) in monolayer at the air-water interface (a) and BAM images obtained during the compression (b) at A = 0.56 nm2 (1), 0.34 nm2 (2), 0.26 nm2 (3), and 0.16 nm2 (4). The scale of the images is 0.35 x 0.30 mm2 [16].
82
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
(1)
(2)
(3)
(4)
Figure 27. Surface pressure-mean molecular area isotherms of 4/8CB mixture (XM = 0.1) in monolayer at the air-water interface (a) and BAM images obtained during the compression (b) at A = 0.46 nm2 (1), 0.30 nm2 (2), 0.21 nm2 (3), and 0.15 nm2 (4). The scale of the images is 0.35 x 0.30 mm2 [16].
Molecular Organization of Thermotropic Liquid Crystals …
83
a) 10
/mNm
-1
8
4
3 2
6 4 2
1
0
0.2
0.3
0.4
A/nm
b)
0.5
0.6
2
(1)
(2)
(3)
(4)
Figure 28. Surface pressure-mean molecular area isotherms of 2/8PCH mixture (XM = 0.1) in monolayer at the air-water interface (a) and BAM images obtained during the compression (b) at A = 0.64 nm2 (1), 0.43 nm2 (2), 0.24 nm2 (3), and 0.15 nm2. The scale of the images is 0.35 x 0.30 mm2 [16].
84
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
(1)
(2)
Figure 29. Surface pressure-mean molecular area isotherms of 2/8PCH at XM = 0.3 in monolayer at the air-water interface (a) and BAM images obtained during the compression (b) at A = 0.26 nm2 (1) and 0.15 nm2 (2). The scale of the images is 0.35 x 0.30 mm2 [15].
The contrast between BAM images recorded behind the collapse point for the dye/liquid crystal mixtures and those for the liquid crystals grows with increasing XM of the dye. Up to XM = 0.5 it is possible to observe in the Langmuir film the creation of small domains, characteristic for given liquid crystal. Upon continuous compression, the number of domains increases, as it is seen in Fig. 29 for 2/8PCH at XM = 0.3. For mixtures of dyes with 8CB the size of domains does not grow, even when two components are miscible. The background monolayer at which the domains of interdigitated bilayer are formed, starts to be rough. As the available area is further reduced, the domains are very close to one another but do not coalesce. It seems that the rough bottom monolayer prevents the formation of structures bigger in the diameter. The mobility of the bilayer created on the rough monolayer is much smaller than in the Langmuir film of 8CB, where the domains of the interdigitated bilayer coalesce easily. It means that the dye molecules are present both in the monolayer and in the upper part of the Langmuir film. This situation remains almost unchanged to the end of the compression process. When for the dye/8CB mixture the phase separation occurs, as in the case presented in Fig. 30 for 4/8CB mixture at XM = 0.3, one notes in BAM images of the mixtures at XM 0.3 small non-regular patches just after spreading the chloroform solution on the water surface. Upon reduction of the available area after the collapse point, the patches grow in size but to the end of the compression process the circular domains are further seen.
Molecular Organization of Thermotropic Liquid Crystals …
(1)
85
(2)
Figure 30. Surface pressure-mean molecular area isotherms of 4/8CB at XM = 0.3 in monolayer at the air-water interface (a) and BAM images obtained during the compression (b) at A = 0.26 nm2 (1) and 0.15 nm2 (2). The scale of the images is 0.35 x 0.30 mm2 [15].
3.2.2. Electronic Absorption Spectra of Langmuir and Langmuir-Blodgett Film
The azo dyes under investigation are characterized by high extinction coefficient (over 20 000 dm3/mol·cm), thus it was possible to measure the absorption of their mixtures with the liquid crystal in the monolayers floating on the water surface (in situ). Figure 31 presents the representative long-wavelength absorption spectra of the Langmuir film of dye 1 mixed with 8CB at XM = 0.3. The spectra were recorded at various surface pressure: before compression (1), at the moment when the surface pressure start to increase (2), below the collapse point (3) and behind this point, when the surface pressure remains constant (4). It can be noticed that there is no significant change in the shape and peak position as the surface pressure is increased. In the case of low XM, the absorbance values were very small and the spectra were strongly noised. Therefore, it was difficult to visualize the maximum position. It succeeded only upon processing the spectra, thus the maxima were identified and they are given in Tables 12-14, together with the half-bandwidth values.
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
86
Figure 31. Long-wavelength absorption spectra in situ of Langmuir film formed of 1/8CB mixture (XM = 0.3) at = 0 (1), 2.5 (2), 6.3 (3), and 8.7 (4) mN/m [16].
Table 12. The position of absorption maximum, max, and the half-bandwidth, , of the long-wavelength absorption band of dyes 1-4 dissolved in ethanol and mixed with 8CB in Langmuir and LB films. Ethanol XM = 1.510-7 Dye max/nm /cm-1 =1nm =10cm-1
a
1
580
3210
2
508
4530
3
486
4720
4
512
4470
- impossible to record,
b
XM 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5
- transfer impossible
8CB Langmuir film LB film max/nm /cm-1 max/nm /cm-1 -1 =1nm =50cm =1nm =50cm-1 612 2850 593 3350 585 3450 598 4150 588 3750 583 4550 568 4100 570 5300 562 4300 560 5550 538 4700 543 5850 -a -a 537 5400 -a -a 518 5850 -a -a -b -b 582 4150 579 5550 546 4600 598 5700 530 5900 575 6950
Molecular Organization of Thermotropic Liquid Crystals …
87
Table 13. The position of absorption maximum, max, and the half-bandwidth, , of the long-wavelength absorption band of dyes 1-4 dissolved in ethanol and mixed with 8PCH in Langmuir and LB films. Ethanol 8PCH XM = 1.510-7 Langmuir film LB film Dye max/nm /cm-1 max/nm /cm-1 max/nm /cm-1 -1 XM -1 =1nm =10cm =1nm =50cm =1nm =50cm-1 0.1 602 3550 587 3350 499 4700 0.3 592 3750 590 4150 1 0.5 590 4300 583 4550 0.1 535 4050 551 4200 481 4800 2 0.3 531 4650 544 5100 0.5 530 5150 533 5900 3 a a 536 3900 0.1 522 4750 0.3 -a -a 524 4950 0.5 -a -a 524 5150 4
a
527
3650
0.1 0.3 0.5
550 550 537
5450 5850 5850
531 531 556
-a 7250 8250
- impossible to record
Table 14. The position of absorption maximum, max, and the half-bandwidth, , of the long-wavelength absorption band of dyes 5-9 dissolved in chloroform and mixed with 8CB in Langmuir and LB films. Chloroform XM = 1.510-7 Dye
max/nm /cm-1 XM =1nm =10cm-1
5
499
4700
6
481
4800
7
536
3900
8
527
3650
9
512
3600
0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5 0.1 0.3 0.5
8CB Langmuir film LB film max/nm -1 /cm max/nm /cm-1 =1n -1 =50cm =1nm =50cm-1 m 534 5050 537 5100 524 5250 529 5150 525 5450 524 5550 520 5000 518 4950 510 5100 504 5400 505 5350 508 5450 560 4500 520 6800 571 4650 522 7250 552 5900 524 7350 535 3800 531 3900 530 4100 531 4350 546 4500 556 4650 520 3900 521 3950 530 4000 534 4100 539 4250 541 4100
The LB films of the dye/liquid crystal mixtures were obtained after deposition of the floating monolayer onto quartz slides at the surface pressure corresponding to the value of
88
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
before the collapse point at the -A isotherm. The absorption spectra were recorded and the positions of the maximum and the half-bandwidths of the long-wavelength absorption band for dyes 1-9 mixed with liquid crystals are gathered in Tables 12-14. For comparison in these tables the data for dyes dissolved in ethanol (dyes 1-4) and chloroform (dyes 5-9) at XM = 1.510-7 are also given. Figure 32 shows normalized absorption spectra of the Langmuir and LB films of 1/8CB (a), 2/8PCH (b), 4/8CB (c) and 4/8PCH (d) mixtures at XM = 0.5, as examples, compared with the spectra of the appropriate dye in ethanol. The solution spectra are characteristic for azo dyes in the monomeric form. In the Langmuir and LB films, the absorption band of dyes 1-9 mixed with the liquid crystal is distinctly broadened in comparison with that in solution (for dye 1 at each concentrations two maxima or maximum with distinct shoulder in 8PCH at higher XM can be distinguished). This observation could suggest that in the monolayers at the air-water and air-solid substrate interfaces some fraction of self-aggregates by dye molecules is created. Indeed neither an additional peak, nor a shoulder, which would indicate the dimer creation in the ground state, is observed, but the dye absorbance in the Langmuir and LB films does not vary proportional to its concentration. This effect can be seen in Figs. 33 and 34. Fig. 33 displays the long-wavelength absorption spectra of 1/8PCH mixture in Langmuir (a) and LB (b) films, whereas in Fig. 34 the UV-Vis absorption spectra of the LB films of 2/8CB and 2/8PCH mixtures at various XM are presented. The band in UV region with the maximum at 280 nm is related to the absorption of 8CB with very small contribution of the dye absorption. For other dyes similar behaviour was found and it can confirm the suggestion about the occurrence of some fraction of 1-9 aggregates in monolayers already in the ground state.
Figure 32. Long-wavelength absorption spectra of Langmuir (1) and LB (2) films of 1/8CB (a), 2/8PCH (b), 4/8CB (c), and 4/8PCH (d) at XM = 0.5. Dashed curve (3) presents a spectrum of a dye dissolved in ethanol at XM = 1.510-7 [16].
Molecular Organization of Thermotropic Liquid Crystals …
89
Figure 33. Long-wavelength absorption spectra of Langmuir (a) and LB (b) films formed of 1/8PCH at XM of a dye of 0.1 (1), 0.3 (2) and 0.5 (3) [16].
The creation of self-aggregates by the azo dye molecules was considered in term of the molecular exciton model, proposed by Kasha et al. [35]. From this model follows that strong interactions among molecules in the aggregate can cause the splitting of the electronic excited state, which appears as a spectral shift of the absorption band and/or its splitting, known in literature as the Davydov splitting [36]. The physical basis of this model is a state interaction theory. In the simplest case, i.e. a binary system composed of two identical molecules or chromophores (dimer), the ground state wave function is expressed by the product of wave functions of molecules u and v:
0 u 0 0 .
(6)
The Hamiltonian operator for the dimer is as follows:
H H u H H u ,
(7)
90
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
Figure 34. Absorption spectra of LB films formed of 2/liquid crystal mixtures at XM of a dye of 0.1 (1), 0.3 (2), and 0.5 (3) for: a) 2/8CB and b) 2/8PCH mixtures [13].
where Hu i Hv are the Hamiltonian operators for individual molecules, and Huv is the term connected with the energy interaction between molecules. Solving the Schrödinger equation, one obtains the following expression for the energy of the ground state of the dimer:
E0 Eu Ev u 0 v 0 H uv u 0 v 0 d u d v .
(8)
The last term represents the van der Waals interaction energy (an energy lowering) between the ground states of molecules u and v, and Eu and Ev are the ground state energies of the isolated molecules (monomers). When each molecule in the dimer undergoes the excitation from the state 0 to the state a, their wave functions of the excited state (exciton wave functions) are represented by the products of two wave functions: of a molecule u in the excited state and a molecule v in the ground state, uav0, and of molecule v in the excited state and molecule u in the ground state, u0va. The wave function of the total system is the linear combination of these two products:
a Cua 0 ua 0 Cu 0a u 0 a .
(9)
Molecular Organization of Thermotropic Liquid Crystals …
91
The Schrödinger equation for the excited state has the following form:
H (Cua 0 ua 0 Cu 0a u 0 a ) E (Cua 0 ua 0 Cu 0a u 0 a ).
(10)
Solving Eq. (10), the following eigen functions and eigen values are obtained:
a 21/ 2 ( ua 0 u 0 0 ),
(11)
E Eua Ev 0 ua v 0 H uv ua v 0 d u d v ua v 0 H uv u 0 va d u d v
(12)
Ea . The last term in Eq. (12) is exciton splitting term, which in the point-dipole point-dipole approximation becomes [31]:
u 0a v0a 3 Ruv
3( u 0 a R )( v 0 a R) 5 Ruv
(13)
and represents an interaction energy due to exchange of the excitation energy between molecule u and molecule v. The third term in Eq. (12) is analogous to the corresponding term in Eq. (8), and represents the van der Waals interaction between an excited molecule u and the ground state molecule v.
u 0 a and v0 a are the electric transition moment of molecules u
and v, respectively, and Ruv is the distance between centers of two molecules. If one takes the difference of the van der Waals interaction energy for the excited and ground states as D, the transition energy for dimer will be the difference between Eq. (12) and Eq. (8):
Edimer E E0 Emonomer D
(14)
This is the characteristic form of the transition energy between ground and excited states of an aggregate, resulting from the exciton model. From Eq. (14) it follows that the interaction between dipole moments of two molecules (chromophores) splits the singly excited state of the dimer into two states, called and states, according to [37], with the following eigen values and eigen functions:
E Ea , a 2 1 / 2 ( ua 0 u 0 0 ),
(15)
E Ea , a 21/ 2 ( ua 0 u 0 0 ).
(16)
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
92
The energy gap between and states, expressed by = 2, is called exciton splitting or Davydov splitting [36]. Figure 35 presents three possibilities of the mutual arrangement of transition dipole moments of two molecules: parallel, in-line, and oblique. In the case (a) the transition to the state is forbidden due to the zero value of the resultant transition moment for antiparallel dipoles arrangement. As a result the maximum of the absorption band is shifted toward shorter wavelengths with respect to the maximum of the appropriate absorption band of the monomer. In the case of in-line alignment (c), the transition to the state is forbidden, which leads to the observation of a spectral red shift for the transition in the dimer compared with that of the monomer. For the oblique alignment (b), the vector sum and difference of two dipole transition moments are always different from zero, giving in the absorption spectrum the band with two maxima.
Figure 35. Exciton band energy diagram for a molecular dimer with parallel (a), oblique (b), and in-line (c) arrangement of the transition dipole moments. The ovals correspond to the molecular profile, and the double arrows indicate the transition dipole moment direction (the transition moment direction need not be parallel to the long molecular axis).
Coplanar arrangement of the transition dipole moments in dimer leads to the exciton energy diagram shown in Fig. 36. This case corresponds to the variation of the angle between the direction of the transition moment of molecules and the line of their centers from 0o to 90o. Thus, = 0o corresponds to the case in Fig. 34c, and = 90o corresponds to the case in Fig. 34a. The energy splitting of the exciton band is now given by the formula [35]:
2 u 0a v0a 3 uv
R
2
(1 3 cos 2 ).
(17)
From Eq. (17) and Fig. 36 it follows that for 0o<<54.7o, the exciton band is energetically located below the monomer band causing a red shift, and created aggregates are called Jaggregates [38]. For 54.7o<<90o, the exciton band is located energetically above the monomer band causing a blue shift, and corresponding aggregates are called H-aggregates [38]. When = 54.7o, no shift in the absorption spectrum is observed, and the aggregates are then called I-aggregates [39].
Molecular Organization of Thermotropic Liquid Crystals …
93
Figure 36. Exciton band energy diagram for dimer with coplanar arrangement of the transition dipole moments.
Looking at the data presented in Tables 12-14 it is seen that the absorption band of all the dyes in the monolayers becomes broader and broader as the dye content increases. However, the shift of the maximum position is different for various dyes. For dyes 1-7 studied at low XM in the Langmuir and LB films the absorption maximum position shifts towards longer wavelengths with respect to the position of the monomeric absorption band. Upon increasing the dye content, the wavelength of the maximum band shortens. Indeed significant differences in the change of the absorption band shape ( and ) at the same dye content in the liquid crystal for various dyes occur, indicating the influence of the molecular structure of the substituents on the spectral properties of the dyes under investigation, but above mentioned behavior of the maximum position for all the mixtures can be noticed. It seems, therefore, that at the change of the dye content in the monolayers at interfaces various kinds of aggregates are formed. One of the possibilities is assumption that at low XM some fraction of Jaggregates is created, whereas at higher concentrations the H-aggregates appear too. We tried to separate the long-wavelength absorption spectra for the azo dye/liquid crystal mixtures under investigation into two or three bands, corresponding to absorption of monomers, Jand/or H-dimers. We supposed that up to the dye molar fraction equal to 10-2, the dye molecules occur only in their monomeric form. Thus, the values of and for the monomer (M) absorption band were taken from the measurements of the absorption of the dyes dissolved in the appropriate liquid crystal at XM = 10-2 in the sandwich cell of 10 m in thickness [13,14,17]. Next, one or two additional maxima were assumed, which should appear at the longer (J-type dimer) and shorter (H-type dimer) wavelengths with respect to the band mximum position of the monomer. A sum of normalized Gaussians as a model function for experimentally obtained absorption band of dye/liquid crystal mixtures in the Langmuir and LB films were used.
94
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
Figure 37 illustrates the exemplary decomposition of the absorption band into Gaussiantype components for 4/8CB mixture at XM = 0.1 (a) and 0.5 (b). The detailed analysis of the data obtained from the decomposition of the absorption spectra of the azo dye/liquid crystal mixtures in LB films is presented in refs. [13,14,17]. For all the mixtures investigated the general observation was made that at low dye content apart from monomers, only J-dimers appear, as in Fig. 37a. When the dye concentration rises, the H-dimers can be also created. In the mixtures of the most dyes with 8CB and 8PCH at XM = 0.5 the monomers, J-dimers and H-dimers in various fractions exist both in the Langmuir and LB films (Fig. 37b). It was found, however, that the mutual orientation of molecules in the aggregate as well as the amount of the appropriate kind of aggregates at given XM strongly depend on the molecular structure of the dye, and first of all on the value and the direction of the resultant dipole moment. For example, for dye 3 the best fitting for the decomposition of the absorption band of its mixture with 8PCH was obtained by assumption that at XM 0.3 only J-type and H-type dimers occur, without presence of the monomers. In the case of dyes 8 and 9 the creation of Jdimers was observed only [17]. With the rise of the dye content more and more aggregates appeared and the amount of the monomers decreased, however H-type dimers were not created. It seems that the direction of the dipole moment in the molecules of dyes 8 and 9 is not conducive to such alignment of the molecules that enables H-dimers creation.
Figure 37. Decomposition of the absorption spectrum of 4/8CB mixture at XM = 0.1 (a) and 0.5 (b) into two (a) and three (b) Gaussian-type absorption bands [13].
Molecular Organization of Thermotropic Liquid Crystals …
95
In order to evaluate quantitatively the orientation of molecules of the azo dyes and the liquid crystals in the monolayer at the solid substrate, the polarized absorption spectra of the LB films were recorded. This kind of measurement was made only for dyes 1-4 mixed with two liquid crystals. Figs. 38 and 39 show examples of the polarized components of the absorption spectra of the LB films of 1/8CB and 4/8PCH mixtures, respectively. For all the mixtures investigated, at the angle of incidence = 0o (see: Fig. 1), both components were equal to each other. This means that the movement of the quartz slide during transfer did not disturb the homogeneity of the molecules arrangement. The shape of the band at 280 nm, related to the absorption of 8CB (Fig. 38), was independent of XM and . However, the AP and AS for the band attributed to the dye absorption had different shapes at various XM and for the mixtures, both with 8CB and 8PCH. As the orientation of monomers and dimers can be, generally, different, the results obtained confirm previous suggestion that in the monolayers at interfaces various kinds of aggregates can be created.
Figure 38. Absorption spectra for light polarized parallel (AP) and perpendicularly (AS) to the incidence plane for 5/8CB mixture as LB film at XM = 0.1 (a) and 0.3 (b). The incidence angle was 60o [13].
96
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
Figure 39. Absorption spectra for light polarized parallel (AP) and perpendicularly (AS) to the incidence plane for 4/8PCH mixture as LB film at XM = 0.5. The incidence angle was 0o (a) and 60o (b) [13].
On the basis of the polarized absorption spectra the angle between the absorption transition moment and the normal to the quartz surface was calculated from Eqs. (2) and (3). Similarly as in the case of the liquid crystals (see: section 3.1.2), it was assumed that the angle between the transition moment direction and the long axis of dyes 1-4, for the longwavelength absorption band, resulting from * transition, is equal to zero. Thus, the angle gives direct information about the orientation of the dye molecules at the quartz surface. Table 15 contains the values of the angle for dyes 1-4 mixed with 8CB or 8PCH in the LB films at XM = 0.1, 0.3 and 0.5. These are the mean values of the results obtained at the angles of incidence, = 30o and 60o, for at least three independently prepared samples. The values of AP and AS were taken at the wavelengths corresponding to the monomer, J-dimer and H-dimer maximum positions, obtained from the best fitting of the Gaussian functions to the experimental spectrum [13,14]. The results obtained indicate that, in general, the angle of all the absorbing species decreases with the rise of the dye content as does the angle between the long molecular axis and the normal to the water surface in the Langmuir films
Molecular Organization of Thermotropic Liquid Crystals …
97
(see data in Tables 10 and 11). However, the value of for a given dye/liquid crystal mixture is greater than that of . This difference can be due to three reasons: (i) the molecular packing can be deteriorated by the stress generated by the transfer of the monolayer from the water surface to the quartz slide, (ii) the methods used to calculate the angles and are different, and (iii) the surface interactions with the water differ from those with the solid substrate. The various angles between the long molecular axis and the normal to the surface in the Langmuir and LB films were found also previously for other dyes [40-45]. The molecular orientation in the LB films strongly depends on the structure of both dye and liquid crystal molecules. For dyes 1 and 4, having a lateral –NO2 group, the greatest values for all absorbing species were observed, indicating that the presence of such group can loosen the molecular packing during the monolayer transfer. Moreover it is seen that, in general, in the mixtures with 8PCH, the molecules are more tilted with respect to the quartz surface than in the corresponding mixtures with 8CB. It is possible that repulsive interactions, observed also in the Langmuir films (see Fig. 22) play here some role. From the data in Table 15 follows that, when the dye molecules form H-type dimers, their long axes show a more vertical orientation with respect to the film surface than in the case of J-type dimers and monomers. Such an observation was made also for other compounds forming self-aggregates in films at interfaces [40]. The greatest angle was obtained for J-type dimers. This seems to be reasonable as these dimers are long and thus not very rigid. One should take also into account that the transition moment direction does not need to be directed along the J-dimer long axis. Conclusions drawn from analysis of the absorption spectra of Langmuir films formed from mixtures of azo dye/liquid crystal allow to propose a model of organization of the molecules in the monolayers at the air-solid substrate interface at low and high contents of a dye. This model is presented in Fig. 40.
Figure 40. Schematic representation of alignment of azo dye and liquid crystal molecules in LB films at low and high concentrations.
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
98
Table 15. Values of the angle, av, between the molecular long axis and the normal to the quartz slide, in LB films of dyes 1-4 mixed with liquid crystals. av/deg Dye/MF 1 XM = 0.1 0.3 0.5 2 XM = 0.1 0.3 0.5 3 XM = 0.1 0.3 0.5 4 XM = 0.1 0.3 0.5
M
8CB H
J
M
8PCH H
J
61 62 43
45 36
62 70 52
62 60 62
66 59
65 66 69
43 43 41
37 38
47 53 49
54 49 50
34 37
55 61 56
60 -
-
62 -
56 -
25 26
60 52 43
43 38 40
45 37
48 50 51
69 62
60 55
70 78
CONCLUSION The thermotropic liquid crystals with rod-shaped molecules are able to create monolayers at the air-water and air-solid substrate interfaces, but this ability strongly depends on the molecular structure of the terminal groups attached to the rigid core of the molecule. The measurements of the surface pressure during compression process of the Langmuir films showed that the liquid crystals with the terminal –NCS group are not able to form a compressible monolayer on the water surface. The mesogenic molecules with very short or very long alkyl or alkoxy chain also do not create Langmuir films. The shapes of the surface pressure-area and surface potential-area isotherms for the Langmuir films of the liquid crystals that make the compressible monolayer at the air-water interface are dependent on the molecular structure of the mesogen rigid core and on the chain length. Brewster angle microscope images revealed that in the case of nematogens giving stable monoayers (4CB6CB, 5OCB, 6OCB, 4PCH-8PCH, 6CPB, 7CPB), behind the collapse point 3D lens-like domains are formed. In the case of smectogens (8CB-10CB) or their precursors (7CB, 7OCB) interdigitated bilayer on the top of the monolayer is formed. Thus, the organization of the liquid crystal molecules in Langmuir films can to some extent be correlated with the type of the mesophase that they form in the bulk. The electronic absorption spectra recorded for the liquid crystals as the LB films indicated that the mesogenic molecules have a tendency to formation of self-aggregates. The polarized absorption spectra of the LB films enabled us to calculate the angle between the long molecular axis and the normal to the quartz surface. Some differences between the molecules tilt angle in the Langmuir and LB films were observed, which can be due to the rearrangement of molecules by the transfer of the floating monolayer on the quartz surface. The different tilt of molecules can be, at least partially, due to the surface interactions of the liquid crystal molecules with the solid surface that are different than with the water.
Molecular Organization of Thermotropic Liquid Crystals …
99
Azo dyes cannot form the Langmuir films themselves, but when one of the thermotropic liquid crystals (here 8CB and 8PCH) was used as supporting matrix, the compression was possible and stable films of azo dye/liquid crystal mixture up to the dye content of at least XM = 0.5 were obtained. The analysis of -A isotherms of the Langmuir films revealed that properties of the monolayer on the water surface (packing density, stability and rigidity) depend strongly on the structure of both the dye and liquid crystal molecules as well as on the mixture composition. The surface potential measurements pointed out that in the spread monolayer, the molecules of the dye are aligned with the dipole moment directed mostly opposite to the dipole moment of the liquid crystal molecules, i.e., from the water to the air. The influence of the miscibility or the immiscibility of both components in the Langmuir film on the change of the surface potential and on the value of the resultant effective dipole moment was found. The electronic absorption spectra recorded for dye/liquid crystal mixtures in both the Langmuir and LB films showed very modest changes with respect to the spectra of the dyes in the diluted solution, primarily in the form of a broadening of the spectrum. The shift of the maximum position of the absorption band, different for various dyes and dependent on the dye molar fraction, was also observed. It was found that in the monolayers at interfaces J-type and H-type aggregates are created by azo dye molecules. The fraction and the type of the aggregates strongly depend on the molecular structure of the dye and can be quite different in both kinds of monolayers. Similarly, as in the case of the liquid crystals, the angle between the long molecular axis of the azo dye and the normal to the solid surface is different from the angle formed with the normal to the water surface. This implies that the molecular packing is loosened during the monolayer transfer. However, some tendency to the tilt angle decrease in H-type dimers and increase in J-type dimers with respect to this angle for monomers can be seen. Such observation indicates that only aggregates in which the transition moment is aligned at high angles (>54.7o-90o) to their line of the centre are able to improve the molecular packing in the LB film.
REFERENCES [1] [2] [3] [4] [5] [6] [7] [8] [9] [10] [11] [12] [13]
Roberts, G. Langmuir-Blodgett Films; Plenum Press: New York, 1990. Janietz, D. In: Handbook of Surfaces and Interfaces of Materials; Nalwa, H.S.; Ed.; Academic Press: New York, 2001; Vol.1, pp. 423-446. Daniel, M.F.; Lettington, O.C.; Small, S.M. Thin Solid Films 1983, 99, 61. Sakuhara, T.; Nakahara, H.; Fukuda, K.; Thin Solid Films 1980, 159, 345. Xue, J.; Jung, C.S.; Kim, M.W. Phys.Rev.Lett. 1992, 69, 474. Friedenberg, M.C.; Fuller, G.G.; Frank, C.; Robertson, C.R. Langmuir 1994, 10, 1251. de Mul, M.N.G.; Mann, J.A. Jr. Langmuir 1994, 10, 2311. Gaines, G.L. Insoluble Monolayers at Liquid-Gas Interface; Interscience: New York, 1996. Martyński, T.; Biadasz, A.; Bauman, D. Liq.Cryst. 2002, 29, 281. Martyński, T.; Miyake, J. Z.Naturforsch. 2003, 58a, 23. Martyński, T.; Biadasz, A.; Bauman, D. Z. Naturforsch.2003, 58a, 97. Bauman, D.; Inglot, K.; Martyński, T. Mol.Cryst.Liq.Cryst. 2007, 479, 49. Inglot, K.; Kaleta, A.; Martyński, T.; Bauman, D. Dyes and Pigments 2008, 77, 303.
Danuta Bauman, Anna Modlińska, and Krzysztof Inglot
100 [14] [15] [16] [17] [18] [19] [20] [21] [22] [23] [24] [25] [26] [27] [28] [29] [30] [31] [32] [33] [34] [35] [36] [37] [38] [39] [40] [41] [42] [43] [44] [45]
Inglot, K. PhD Thesis, Poznań 2008 (in Polish). Inglot, K.; Martyński, T.; Bauman, D. Dyes and Pigments 2009, 80, 106. Inglot, K.; Martyński, T.; Bauman, D. Opto-Electronics Review 2009, 17, 120. Bauman, D.; Płóciennik, A.; Inglot, K. Acta Phys.Polon.A 2009, 115, 203. Organic molecular aggregates: Electronic Excitation and Interaction Processes; Reineker, P.; Haken, H.; Wold, H.C.; Eds.; Springer: Berlin, 1983. Side-chain Liquid Crystal Polymers; Mc Ardle, C.B.; Ed.; Blackie: Glasgow, 1984. Davies, J.T.; Rideal, E.K. Interfacial Phenomena; Academic Press: New York, 1963. Myers, D. Surfaces, Interfaces and Colloids; Willey-VCH: New York, 1999. Hoenig, D.; Moebius, D. J.Phys.Chem. 1991, 95, 4590. Inglot, K.; Martyński, T.; Bauman, D. Liq.Cryst. 2006, 33, 855. Modlińska, A.; Inglot, K.; Martyński, T.; Dąbrowski, R.; Jadżyn, J.; Bauman, D. Liq.Cryst. 2009, 36, 197. Martyński, T.; Hertmanowski, R.; Bauman, D. Liq.Cryst. 2001, 28, 437. Martyński, T.; Hertmanowski, R.; Bauman, D. Liq.Cryst. 2002, 29, 99. Schmitz, P.; Gruler, H. Europhys Lett. 1995, 29, 451. Demchak, R.J.; Fort, T.J., Jr. J.Colloid Interface Sci. 1974, 46, 191. Dynarowicz-Łątka, P. Adv.Colloid Interface Sci. 1993, 45, 215. Oliveira, O.N., Jr.; Taylor, D.M.; Lewis, T.J.; Salvagno, S.; Stirling, C.J.M. J.Chem.Soc. Faraday Trans. 1989, 85, 85. Taylor, D.M.; Baynes, G.F. Mat.Sci.Engng.C 1999, 8-9, 65. Suresh, K.A.; Bhattacharyya, A. Langmuir 1997, 13, 1377. N‟Soukpoé-Kossi, Ch.N.; Sielewiesiuk, J.; Leblanc, R.M.; Bone, R.A.;. Landrum, J.T. Biochim.Biophys. 1988, 940, 255. Angelova, A.; van der Auweraer, M.; Ionov, R.; Vollhardt, D.; de Schryver, F.C., Langmuir 1995, 11, 3167. Kasha, M.; Rawls, H.R.; Ashraf El-Bayoumi, M. Pure Appl.Chem. 1965, 11, 371. Davydov, A.S. Theory of Molecular Excitons; Mc Graw-Hill Book Company, Inc.: New York, 1962. Harada, N.; Nakanishi, K. In: Circular Dichroism Spectroscopy – Exciton Coupling in Organic Chemistry; University Science Books: Mill Valey, CA, 1983. Moebius, D. Adv.Mat. 1995, 7, 437. Miyata, A.; Heard, D.; Unuma, Y.; Higashigaki, Y. Thin Solid Films 1992, 210/211, 175. Kawai, T.; Umemura, J.; Takenaka, T. Langmuir 1989, 5, 1378. Johnson, E.; Aroca, R.; Nagao, Y. J.Phys.Chem. 1991, 95, 8840. Hertmanowski, R.; Chudziński, Ł.; Martyński, T.; Stempniewicz, P.; Wolarz, E.; Bauman, D. Liq.Cryst. 2004, 31, 791. Biadasz, A.; Martyński, T.; Stolarski, R.; Bauman, D. Liq.Cryst. 2004, 31, 1639. Biadasz, A.; Martyński, T.; Stolarski, R.; Bauman, D. Liq.Cryst. 2006, 33, 307. Bielejewska, N.; Chrzumnicka, E.; Stolarski, R.; Bauman, D. Opto-Electronics Review 2010, 18,197. Reviewed by Prof. Dr. Piotr Bojarski, Institute of Experimental Physics, University of
Gdańsk, Poland.
In: Langmuir Monolayers … Editors: Jennifer A. Sherwin
ISBN: 978-1-61122-461-0 ©2011 Nova Science Publishers, Inc.
Chapter 3
ATOMIC FORCE MICROSCOPY CHARACTERIZATION OF LIPID/PROTEIN NANOSTRUCTURES FORMED IN LANGMUIR-BLODGETT FILMS Yih Horng Tan and Keith J. Stine Department of Chemistry and Biochemistry and Center for Nanoscience, University of Missouri – Saint Louis, Saint Louis, MO
ABSTRACT Recently, much of the emphasis in biotechnology has been on producing nanosystems and nanodevices for a vast range of medical applications, including nanoelectronic biosensors, drug delivery systems, and diagnostic and imaging techniques, to name a few. This chapter reviews the potentially useful creation of proteo-lipidic nanostructures generated via the Langmuir-Blodgett (LB) film method, and their direct characterization by atomic force microscopy (AFM). Following the introductory sections, a brief overview on LB film fabrication on surfaces suitable for AFM will be presented, LB films containing proteins, lipids, and biocompatible amphiphilic molecules will be described, and how they have been studied using various AFM imaging modes. We aim to highlight recent developments that illustrate the unique capability of AFM in elucidating nanometer scale organization and the physicochemical properties of artificially engineered biological membranes through the Langmuir-Blodgett method; as it could potentially open a new pathway toward the development of self-organized nanostructures of technological significance.
INTRODUCTION The utilization of biological molecules such as enzymes, peptides or antibodies concurrently with artificially engineered amphiphilic lipid monolayer films to elucidate the origin, composition, size and lifetime of microdomains in biological membranes has been the subject of scientific curiosity for most of the past three decades. In this respect, LangmuirBlodgett (LB) monolayers at the air/water (A/W) interface incorporating proteins are
102
Yih Horng Tan and Keith J. Stine
promising model systems that can be used to correlate the relationship between artificial structures and natural biological membranes. The imitation of natural biological membranes using proteo-lipidic LB model systems is made possible by introduction of biomolecules into the amphiphilic LB films. This approach to understanding biological activities, including biospecific recognition properties, may yield improved insight into these processes and provide the basic understanding needed for many applications in nanobiotechnology that are poised to play a major role in next-generation drug delivery systems, signal detection, biosensors and molecular labeling technology.[1-12] There have been some excellent detailed reviews of the development of biomimetic and functional proteo-lipidic nanostructures based on Langmuir-Blodgett technology over the past few years.[6-8, 11-16] For example, Godoy et al. demonstrated that the ability to control the molecular architecture of LB films was essential for preparing a biosensor with a highly organized proteo-lipidic structure able to partition a non-inhibitory monoclonal antibody in a functional orientation in order to bind an enzyme in an active and stable orientation.[15] In another paper from the same group (Girard-Egrot et al. in 2003), it was shown that the parameters which influence the kinetics of the surface film formation can affect the orientation of the immunoglobulin G, when it is inserted into a mixed glycolipid monolayer formed by spreading of proteo-glycolipid vesicles.[16] Along with the rapid progress in understanding the molecular organization of amphiphiles in LB films, and their association with proteins/enzymes, many optical microscopy techniques have been used to gain insight into the morphological texture, lattice structure, phase behavior and the molecular structure of amphiphilic monolayers.[17-18] Similarly, Brewster angle microscopy (BAM), has been used to reveal that amphiphilic monolayers can self-assemble into mesoscopic domain structures, and the introduction of synchrotron X-ray diffraction at grazing incidence (GIXD) has made possible the determination of two-dimensional lattice structures.[14, 19-20] Furthermore, examples of membrane microdomains resulting from lipid-protein, lipidlipid and protein-protein interactions were reported by using fluorescence photobleaching recovery, fluorescence digital imaging microscopy and single molecule fluorescence microscopy.[12, 21-23] Among all the available surface analysis tools and above mentioned techniques, atomic force microscopy (AFM) was also applied to investigate the amphiphilic monolayer films generated via the LB technique.[24-25] Many high molecular resolution images of single component LB monolayers and multilayers were reported recently.[26-27] For example, by preparing a LB film of a 1:1 molar mixture of arachidic acid and a partially fluorinated carboxylic acid, Gotoh et al., showed that phase separation in multicomponent LB films can be revealed using both AFM normal and lateral force imaging. In their report, the vertical resolution of the domain topography identified reached a resolution of approximately 5Å and the typical lateral dimension of the round shaped domains ranged from 100 nm to 1 m in diameter. Further, the chemical makeup of each phase was able to be assigned by making reference to the frictional information acquired on the surfaces of LB films of the pure components.[28] Also in connection with biological applications, aside from visualizing objects on a surface at nanometer scale, AFM is capable of in-situ surface manipulation followed by insitu measurements, and real time data acquisition.[29-38] Niehus et al. reported the morphology and the stability of supported LB films of phospholipids such as 1,2-dipalmitoylsn-glycero-3-phosphocholine, 1,2-dimyristoyl-sn-glycero-3-phosphocholine and 1,2-dioleoyl-
Atomic Force Microscopy Characterization …
103
sn-glycero-3-phosphocholine/1,2-dipalmitoyl-sn-glycero-3-phosphocholine (DPPC, DMPC, and DOPC/DPPC, respectively) layers, and demonstrated that using AFM is suitable for studying time-dependent biological and physical phenomena.[38] Other applications of AFM also extended to examining phospholipid layers supported on various solid substrates, such as mica or glass, characterizing vesicle fusion and membrane lithography via lipid backfilling methods, and AFM anodization lithography on specialized resists using amphiphilic molecules of hexadecylamine (HDA) and palmitic acid (PA).[38-44] In this review chapter, we aim to highlight the nanometer scale organization and the physicochemical properties of artificially engineered biological membranes elucidated by using AFM; in particular, high resolution imaging of biologically relevant thin films that extends from the molecular to the microscopic level. Studies using real-time AFM imaging techniques illustrating (i) the effect of lipidic LB films upon protein adsorption, (ii) the stability of proteo-lipidic LB films, and (iii) the kinetic behavior of immobilized proteins/drug complexes in a biomimetic environment via real-time AFM imaging techniques will be discussed to emphasize the information that AFM can provide. A brief discussion of a variety of recent AFM imaging techniques or developments will be presented, that might open new avenues in model and biomembrane AFM applications.
LANGMUIR-BLODGETT TECHNOLOGY Langmuir-Blodgett films with proteo-lipidic nanostructures have been extensively used as model membrane systems in biophysics to study/investigate biocatalytic or biomimetic phenomena.[7-8, 45] The use of Langmuir-Blodgett films is possible due to the natural properties of organic molecules such as fatty acids, phospholipids, glycolipids, sterols, etc, that can orient themselves at the air/water interface. Traditionally, the molecules forming Langmuir monolayers are amphiphilic molecules that contain both hydrophilic and hydrophobic structural regions. The hydrophilic (water loving) end typically is either charged or contains a polar head group. In contrast, the hydrophobic (water hating) end typically is nonpolar and not easily dissolved in water.[46] In general, all amphiphiles are potentially ideal materials for monolayer formation. Regardless of whether they are naturally occurring or synthetic, these molecules will spread/accumulate at the air/water interface. The strength of their affinity to the air/water interface, is determined by the balance of hydrophilic and hydrophobic components in their structure, directly determines the physicochemical properties of the monolayers formed. Figure 1 illustrates Langmuir-Blodgett monolayer formation by typical lipid amphiphiles having two hydrocarbon chains and a head-group. At a controlled initial condition just after spreading (from a dilute amphiphile solution in a spreading solvent such as chloroform), the average separation distance between molecules is large and the lateral molecular attractions are usually at a minimum, as depicted in Figure 1A. The available surface area in the Langmuir-Blodgett trough is then decreased by applying compression using the moving barrier, and the average distance between molecules decreases, as depicted in Figure 1B. Continuing to increase the compression can lead to a highly organized monomolecular monolayer at the air/water interface, as depicted in Figure 1C. The formation of a highly organized monolayer upon compression depends upon the amphiphile structure, including
104
Yih Horng Tan and Keith J. Stine
variables such as the chain length. For example, the phospholipid DPPC (two C16 chains) forms an ordered liquid-condensed phase (LC) upon compression at room temperature, while the phospholipid DMPC (two C14 chains), remains in a liquid-like liquid-expanded phase (LE) even at the full extent of compression.[47] Further compression will result in monolayer collapse into the third dimension, by a variety of mechanisms, as has been recently reviewed.[48] Wilhelmy's surface balance Amphiphiles
A
Floatation device
0 mN/m Water
Langmuir Blodgett Trough
B
Compression
Langmuir Blodgett Trough
C
40 mN/m
Compression
Langmuir Blodgett Trough
Figure 1. Langmuir Monolayer Formation. (A) Amphiphiles not yet under any external compression by floating barrier device. (B) Some molecular interaction and initial organization of amphiphiles occurs when film compression is initiated by the floating device. (C) Well-ordered Langmuir monolayer formed, at elevated surface pressure.
SURFACE PRESSURE AND ITS RELATION TO SURFACE TENSION As discussed in greater detail elsewhere, water molecules at the air/water interface possess an excess free energy originating from the difference in environment between the surface molecules and those in the bulk.[6, 12, 49] This interfacial free energy is accessible by measurements of the surface tension, denoted as (). When amphiphilic molecules are spread on the water surface, the formation of a Langmuir monolayer will affect, and in particular decrease, the surface tension.[6, 46] This change in surface tension occurs because when amphiphilic molecules (primarily the hydrophobic ends) are in close proximity, interaction and exertion of repulsive forces among the molecules occurs. The force exerted by the film is referred to as the surface pressure () and is equal to the reduction of the surface tension of the pure liquid subphase by the film, and is given by the following relationship
Atomic Force Microscopy Characterization …
105
o where γo represents the surface tension of the pure liquid subphase and γ represents the surface tension in the present of amphiphiles. The surface tension of pure water is 72.8 mN m1 at 20 oC and depends slightly on the addition of electrolytes.
SURFACE PRESSURE VERSUS AREA ISOTHERMS Traditionally, the primary method used to evaluate and monitor the Langmuir film properties of a given amphiphilic molecule is by measuring surface pressure versus mean molecular area isotherms. In the isotherm measurement, essential information such as the total number of molecules spread on the water surface at a given area is known, the experiment is carried out at a constant controlled temperature, and the subphase conditions are specified (pH, electrolyte concentration, concentrations of other dissolved species). Classically, the area per molecule, which represents the mean area available to each molecule, is calculated by dividing the film area (determined by the barrier position during the compression) by the total number of molecules spread on the water surface.[8] The area per molecule, A, is typically expressed in Å2/molecule or nm2/molecule. A characteristic surface pressure versus area (π-A) isotherm is shown in Figure 2. Maximum surface pressure reached before collapse mechanisms become dominant
Surface Pressure, π (mN/m)
80 70
Collapse phase Water
60
Solid Phase (S)
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
LC/ S
50 40
Water
-+ -+ -+ -+ -+ -+ -+
Liquid Condensed, (LC)
LE /LC
Water
30 LE - LC
-+
20 10
-+
Water
LE
-+
-+
- + +-
Nonpolar tail
Liquid Expanded, (LE) Gas Phase, (G)
-+
G
-+
Polar head
Water
50 100 Area per molecule, ζ (Å2/molecule)
Figure 2. Surface pressure (π-A) isotherm for a lipid with distinct phase regions of differing compressibility. The isotherm curve represents a typical surface pressure versus area per molecule dependence at a fixed temperature, and often shows sharp bends or kinks to indicate the phase transitions occurring in the two dimensional layer at the air/water interface. The isotherm shown is typical for a phospholipid that forms a condensed phase.
The π-A isotherm in Figure 2 indicates a number of distinct segments; these segments correspond to the presence of different two-dimensional phases. When a monolayer is compressed it can go through several diverse phases. The phase behavior of the monolayer is
106
Yih Horng Tan and Keith J. Stine
based on the physicochemical properties of the amphiphilic molecules, at constant temperature, subphase pH, surface pressure, and other subphase variables. It is worth noting that the hydrophobic and hydrophilic regions of amphiphiles each play critical roles. An increase in the chain length of the hydrophobic group will result in increased attraction between molecules and favor the formation of more ordered condensed phases. The cohesive and repulsive forces will change if an ionizable or charged amphiphile are used, and the presence of charged head groups generally makes the formation of condensed phases less favorable. Conventional terminology used to classify different phases has been adopted.[13] The gaseous phase (G) typically represents the largest areas per molecule, with small molecular interactions and minimum to no lateral cohesion in the monolayer. When compressed, the hydrophobic ends of the amphiphiles will start to experience some lateral cohesion; however, the hydrophilic ends of the amphiphiles will remain randomly oriented. This phase is known as the liquid-expanded phase (LE), as show in Figure 2. Continued compression of the LE phase will, for certain chain lengths and depending on temperature, result in a first-order phase transition during which the liquid-condensed (LC) phaseemerges. This first-order phase transition has a broad coexistence region signified by a quasi-plateau in the surface pressure. The LE-LC coexistence region is analogous to the coexistence of liquid and vapor phases in three-dimensions and the proportion of the two phases at points along the isotherm within this segment is governed by the thermodynamic lever rule. The LC phase is characterized by a significant degree of chain ordering together with only short-range positional ordering of the head-groups. LC phases can have either vertically oriented or tilted chains, and transitions between tilted and vertical phases are possible. Upon compression out of the plateau-like segment, the LE phase is completely converted to the LC, and at even higher densities the monolayer finally reaches the solid phase (S), in which the molecules are closely packed and highly ordered both in terms of chain orientation and head-group positional ordering. If the monolayer is further compressed after reaching the S phase, the monolayer will collapse into three-dimensional structures (as illustrated on the right side of Figure 2 at the top).
LANGMUIR-BLODGETT FILM DEPOSITION Langmuir-Blodgett films are generated by a successive deposition process in which a monolayer on the water surface is transferred onto a solid substrate. This process was demonstrated by Dr. Katherine Blodgett, in 1935, after the introduction of the Langmuir film by Dr. Irving Langmuir in 1917. The deposition process require surface pressure, temperature, pH, and other parameters be controlled at constant values while the transfer process is accomplished by successively dipping a solid substrate up or down at a controlled rate through the surface monolayer, as depicted in Figure 3. The solid substrate may start the process either held above the air/water interface and ready for the immersion (down stroke), or immersed and ready to be pulled out at a fixed rate (upstroke). If the substrate is hydrophobic, as is the case for chemically modified gold or silicon, the substrate will be positioned above the surface and ready for a down stroke. If the substrate is hydrophilic, such as a clean glass slide, the substrate will be position immersed into the subphase and ready for the first upstroke. When the substrate is hydrophilic and starts out immersed, the subphase
Atomic Force Microscopy Characterization …
107
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
C
-+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
D
-+ -+
Hydrophobic Substrate
B
A -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
Hydrophilic Substrate
will wet the substrate and the contact angle will be near zero at the three-phase contact line, which represents the border where monolayer transfer occurs during substrate motion. The monolayer will naturally flow onto the substrate as it is raised in this case and transfer in a head-groups down orientation. For hydrophobic substrates, the aqueous subphase does not wet the substrate and the contact angle will be near 180o upon immersion, facilitating transfer in a tails-down orientation. The degree of success in transfer is expressed in the form of the transfer ratio, defined as the ratio of the decrease in area of the monolayer on the water surface divided by the substrate area. Perfect transfer of a stable monolayer at constant surface pressure will result in a transfer ratio of unity.
-+ -+ -+ -+ -+ -+ -+
Figure 3. Langmuir-Blodgett Deposition (see text for detailed discussion). (A) Deposition onto a hydrophilic substrate during emersion, (B) deposition of the second layer during immersion, (C) deposition onto hydrophobic substrate during immersion, and (D) deposition of the second layer during emersion.
When the substrate is hydrophilic, during the first upstroke the very first monolayer transferred onto the substrate will orient with its hydrophilic head-groups interacting with the substrate. When the first transfer step is completed, the initial hydrophilic substrate becomes hydrophobic as it is now covered by a monolayer with hydrocarbon chains oriented towards the air. If the motion of the dipper is reversed and a subsequent immersion step is now carried out, the newly formed hydrophobic outermost layer will attract the hydrophobic chains of the surface-monolayer, as seen in Figure 3B. The result will be a bilayer structure. Continuing the deposition process (emersion and immersion of substrate) will lead to multiple layers of monomolecular amphiphiles of alternate orientation. This process is known as Y-type deposition, as shown in Figure 4 (for the case of a hydrophilic substrate). If the substrate is hydrophobic, the first monolayer will transfer tails-down on the first immersion and as the substrate is pulled out, the second layer will transfer with the headgroups interacting with those of the first monolayer. The result after multiple cycles of
108
Yih Horng Tan and Keith J. Stine
immersion and emersion resulting in multilayer formation will still be Y-type deposition, but with the first monolayer being tails-down instead of heads-down.
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
Y-type deposition
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
X-type deposition
C -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
B -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
-+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+ -+
A
Z-type deposition
Figure 4. X-, Y- and Z-type multilayers.
Besides the Y-type deposition, two other monolayer deposition orientations on solid substrates have been reported.[6, 46] X-type results from transfer only upon immersion steps and the resulting layers are all oriented in the same manner with the tails pointing towards the substrate. Z-type deposition occurs only on emersion steps and yields multilayers whose individual monolayers are all oriented with the head-groups pointing towards the substrates. It has been reported that the X- or Z-type deposited multilayers, as indicated by the transfer ratios, sometime rearrange into a Y-type repeating bilayer organization.[50] The above mentioned deposition types (or modes), can be influenced by many factors, such as the nature of the amphiphiles, transfer surface pressure, deposition speed, pH, temperature, packing of the monomolecular layer at the air/water interface, and the presence of dissolved subphase cations that interact with the head-groups.[51-55] Langmuir-Blodgett films can be formed by transfer of phospholipid monolayers, and also by transfer of phospholipid mixed monolayers or phospholipid-cholesterol mixtures. It is possible to transfer single monolayers, bilayers, or multilayers.[56] The transfer of multilayers of DPPC is not easy but has been enhanced by addition of DPPA (dipalmitoylphosphatidic acid) as a transfer promoter. It has been reported that for transfer onto hydrophilic substrates, transfer of the first layer is generally possible with transfer ratio of nearly 1.0; however, successful transfer of the second layer was noted as being successful only in a narrow range of surface pressure.[57] It is also possible to transfer a different phospholipid in the second layer than in the first. In a study making use of AFM, Kruijff et al. revealed that when the first layer was DPPC, AFM topographic image indicated that DPPC in general looked smooth with a few small defects, as seen in Figure 5A.[58] Furthermore, when the second layer was DPPC, the films appeared relatively smooth with a small number of round defects covering less than 6% of the surface, as seen in Figure 5B. These features were well below the resolution limit of optical microscopy methods such as fluorescence microscopy. Futhermore, Kruijff et al. also indicated the shape of the defects in asymmetric LB bilayers was influenced by the nature of the first leaflet; for example, polygonal lineshaped defects were observed in 1,2-dipalmitoyl-sn-glycero-3-phosphocholine/1,2dipalmitoyl-sn-glycero-3-[phospho-rac-(1-glycerol)] (DPPC/DPPG) bilayers. Again, the irregularly shaped features continued to be present and display elevations from the rest of 1,2-
Atomic Force Microscopy Characterization …
109
dipalmitoyl-sn-glycero-3-phosphocholine/1,2-dimyristoyl-sn-glycero-3-[phospho-rac-(1glycerol)] (DPPC/DMPG) bilayers as illustrated in Figure 5C and 5D (second layer leaflets of the bilayer are in the condensed phase). Whereas mainly line-shaped, polygonal features and some small irregularly shaped defects were seen when 1,2-dimyristoyl-sn-glycero-3[phospho-rac-(1-glycerol)] (DMPG) or 1,2-dioleoyl-sn-glycero-3-[phospho-rac-(1-glycerol)] (DOPG) were used as a second layer in the bilayer system, as seen in Figure 5E and 5F (second layer leaflets of the bilayer are in the liquid phase).[58]
Figure 5. Morphology of LB Phospholipid Layers Revealed by AFM. (A) Monolayer of DPPC (condensed phase), transferred at a surface pressure of 35 mN/m. Such a monolayer was used as the first leaflet of the following bilayers, of which the second leaflet was transferred from 10 mM Tris buffer, with 100 mM NaCl, pH 7.4, and consisted of (B) DPPC deposited at a surface pressure of 26 mN/m (condensed phase); (C) DPPG deposited at 26 mN/m (condensed phase); (D) DMPG deposited at 35 mN/m (condensed phase); (E) DMPG deposited at 22 mN/m (liquid-expanded phase); and (F) DOPG deposited at 26 mN/m (liquid-expanded phase). All images are 10 m x 10 m; scale bar = 2 m; z-scale is 10 nm. (see original article, de Kruijff, B. 1999). Reprinted with permission from reference 58.
110
Yih Horng Tan and Keith J. Stine
MOLECULES THAT FORM BIOMIMETIC MONOLAYERS In theory, any compound or molecule possessing both hydrophilic and hydrophobic properties is a good candidate for monolayer formation. Many of the common amphiphiles, such as fatty acids, cholesterol, glycolipids, phospholipids, and others, are commonly used to prepare Langmuir-Blodgett films, because they have the potential to serve as biomimetic membranes. The structures of some of the molecules most commonly used to form biomimetic membranes are shown in Figure 6.[54-55, 59-68]
Sphingomyelin
Digalactosyl diglyceride
Phosphotidylglycerol
Diphosphotidyl glycerol
Cholesterol
Galactosylceramide
Sphingolipids
Glycolipids Monogalactosyl diglyceride
Phosphotidylserine
Phosphotidylinositol
Phosphatidylethanolamine
Phosphatidylcholine
Phospholipids
Figure 6. Representative structures of some of the main membrane lipids that are potentially of interest for formation of Langmuir-Blodgett films acting as biomimetic membranes.
The hydrophobic portions of the amphiphilic molecules prevent water solubility, while the hydrophilic ends interact favorably with water. It is crucial that there be an appropriate balance between the head-group hydrophilicity and the hydrophobicity of the hydrocarbon chains for successful monolayer formation. If the hydrocarbon region is too short, the amphiphilic molecules will simply dissolved in the subphase shortly after spreading. A general rule of thumb, for the spreading of single saturated chain derivatives, is that a minimum hydrocarbon chain length of 12 ((-CH2-)n, n ≥12) is necessary to ensure that the hydrocarbon chain is long enough for the compound to form a spread monolayer that remains at the air/water interface long enough for most experiments.[6, 14] Monolayers are thermodynamically metastable systems, and should ultimately dissolve into the subphase; however, they do so extremely slowly if the chain length is sufficient long. It is also worth noting, introduction of a double bond (either cis or trans conformation, Figure 7A and B, respectively) into the middle of the hydrocarbon chain will significantly disrupt the molecular packing of the Langmuir firm and change the surface area per molecule and ability to undergo
Atomic Force Microscopy Characterization …
111
deposition onto substrate surfaces, especially for cis double bonds in the middle of the chain. On the other hand, disruption of the molecular packing is minimal if the double bond is at the end of hydrocarbon chain, as seen in Figure 8.[46]
B
A
Oleic acid Figure 7. Structures of Oleic Acid and Elaidic Acid.
Tricosenoic acid Figure 8. Structure of Tricosenoic acid.
Elaidic acid
112
Yih Horng Tan and Keith J. Stine
For the case of phospholipids and related two-chain amphiphiles, monolayer formation can sometimes be successful for chain lengths shorter than 12 –CH2 units.[69] For example, the surface pressure-area isotherms of 1,2-didecanoyl phosphatidylcholine and 1,2-didecanoyl phosphatidylethanolamine were reported in early studies. Such shorter chain length phospholipid derivatives form highly fluid monolayers which have featureless isotherms showing smoothly increasing surface pressure and high compressibility.[70] LangmuirBlodgett films of these very short phospholipids have not been reported. Under ambient conditions, the phospholipid DMPC is in the liquid-expanded phase, and increasing the chain length by two –CH2 units to C16 in DMPC results in a monolayer that is in the liquidcondensed phase at ambient conditions and surface pressures of most interest for LB transfer.
LIPID/PROTEIN LANGMUIR-BLODGETT FILMS The LB technique offers one of the best possibilities to perfectly control each step of the film preparation, largely due to the molecular arrangement and perfectly organization at the air/water interface. The molecular packing itself is robust and can be maintained during the transfer process onto the desired solid support, when all the parameters are optimized. In the context of biomimetic studies, LB films composed of phospholipids, such as 1palmitoyl-2-oleoyl-sn-glycero-3-phosphocholine (POPC) [71] and 1,2-dipalmitoyl-snglycero-3-phosphocholine (DPPC),[71] other phosphatidylcholines,[72-75] phosphatidylethanolamines, [76] etc, are a few of the many essential components of biological membranes of interest. The functionalization of LB films with biological molecules can be achieved by association with proteins presenting specific recognition properties, for example, enzymes, antibodies or bio-specific ligands. In the past decades, utilization of biomolecules such as enzymes or antibodies in conjunction with amphiphilic molecules via LB thin film approaches have been reported and several bioactive protein-lipid LB films have been studied with regard to their potential application in biosensor development. [4, 6, 77-83] The popularity of this approach is mainly due to the ease of preparation and incorporation of biological molecules that act as models for biological membrane structures or functions, and may be used for studying and testing isolated functions by systematic control of composition. Some crucial and lingering questions (to name a few) include: (i) determination of the minimum amount of enzyme needed for membrane preparation for biosensor function; (ii) whether one-step preparation of a bioactive sensing layer and its association with the transducer is possible; (iii) the possibility to work at ambient environmental conditions (atmospheric pressure and temperature) to avoid denaturing the biological compounds; (iv) the ability to modulate the sensor performance (detection limit, sensitivity, dynamic range) by varying the number of the deposited proteolipidic layers.[77, 84-89] The resolution of these issues remain vital for further development or design of microscale or nanoscale sensors capable of operating in controlled environments and with ultra-rapid response times. Several methodologies for incorporation of proteins, enzymes, or biological compounds into LB films have been reported including: (i) adsorption of protein from the subphase onto the interfacial film by means of spreading the monolayer onto a subphase containing the dissolved protein or by injecting the protein into the subphase after lipid monolayer
Atomic Force Microscopy Characterization …
113
formation,[77, 80-82, 84-86, 89-108] (ii) adsorption of the protein onto the LB film after transfer, and (iii) co-spreading of protein included in the spreading solution just prior to LB monolayer formation has also been reported.[4, 109-110] Although many successful incorporations of protein in LB monolayers have been reported, the presence of protein in LB monolayers in general can modify the packing of the amphiphile at the air/water interface and inevitably complicate the transfer procedure onto a solid support.[89, 104, 111] These complications could be attributed to the fact that protein incorporation changes the surface pressure behavior of the monolayer and its stability, can induce poor monolayer adhesion to the solid support which can lead to peeling off during subsequent immersion/deposition steps, and release of protein molecules into the subphase during deposition due to their weak association with the amphiphilic molecules, etc.[112-113] The reported strategies to overcome the above mention problems, include but are not limited to: (i) usage of a covalent binding approach, to directly immobilize protein onto the cross-linking agents in the LB film,[114-115] (ii) stabilization the proteo-lipidic monolayer by using glutaraldehyde vapour as a protein cross-linker,[81-82, 104] and, (iii) stabilizing the choline oxidase enzyme in the proteo-lipidic LB film by using the heads of the two opposing lipidic layers (referred to as inclusion by sandwiching).[7, 116-117]
PROTEIN ORIENTATION OR DIRECTED PROTEIN PRESENTATION With the ultimate goal of biomimetic membrane applications in nanobiotechnology, understanding and controlling macromolecule presentation and orientation in proteo-lipidic nanostructures intended for use in biocatalysis or based on biomolecular recognition by the immobilized biological macromolecules, e.g. enzymes, antibodies, etc., is crucial for the success of innovative strategies in the future development of integrated nanobioelectronic devices. Many strategies have so far been reported to incorporate proteins in LB layer(s) and to build stable proteo-lipidic LB films onto solid supports. The control of the protein incorporation and presentation in a defined orientation that mimics that in a natural biological membrane to achieve maximum functionality is important and remains one of the many challenges in designing proteo-lipidic LB layer(s) for biomimetic sensing applications. To meet these challenges, numerous systematic tactics have been reported in the past decades, towards the goal of generating oriented proteins in lipidic LB films. One of the methods involved covalently associating antibody fragments to lipids bearing thiol or lipoyl head-groups via disulfide bonds to the free thiols formed after the hinge regions of the immunoglobulins had been cleaved by the enzyme pepsin. A different approach used histidine tag containing proteins associated onto monolayers of lipids bearing Ni2+ chelating head-groups.[118-121] An alternate approach reported by Girard-Egrot et al., involved inserting a non-inhibitory monoclonal antibody in LB films as a form of anchor, thus the hydrophilic protein can be associated in an oriented position at the surface of lipidic matrix.[15] In fact, the reported strategy by Girard-Egrot et. al., was also capable of increasing the shelf life of the proteo-lipidic LB films and retain the biological activity of the immobilized proteins, for up to few months.[45] In this study, activity of the
114
Yih Horng Tan and Keith J. Stine
acetylcholinesterase monomers (AChE), in an orientated position, at the surface of the IgGglycolipid LB film after immunoassociation was demonstrated. Furthermore, the approach of incorporating biological molecules, such as proteins, in liposomes and the applying Langmuir-Blodgett techniques was successful. The proteo-lipidic vesicle can be spread onto the air/water or air/buffer interface in the Langmuir Blodgett trough. Upon the disintegration of the proteo-lipidic liposomes, the proteo-lipidic LB films can be generated by compressing the film up to the transfer surface pressure (eg: 30 mN/m) and then transferring onto the solid support.[16, 122-128]
AFM CHARACTERIZATION OF SUPPORTED BILAYERS For the characterization of the monolayers at the air/water interface that are the precursors to LB films, many advanced and promising techniques such as fluorescence microscopy and fluorescence recovery after photobleaching (FRAP) methods[129-130], Brewster-angle microscopy (BAM), x-ray and neutron scattering techniques, external reflection Fourier transform infrared (FTIR) spectroscopy, and polarization-modulated infrared reflection absorption spectroscopy (PM-IRRAS) have been applied.[131-135] The above mentioned