EMC 2008 14th European Microscopy Congress 1–5 September 2008, Aachen, Germany
Sivia Richter · Alexander Schwedt Editors
EMC 2008 14th European Microscopy Congress 1–5 September 2008, Aachen, Germany Volume 2: Materials Science
13
Dr. Silvia Richter Dr. Alexander Schwedt RWTH Aachen Central Facility for Electron Microscopy Ahornstr. 55 52074 Aachen Germany
[email protected] [email protected]
ISBN 978-3-540-85225-4
e-ISBN 978-3-540-85226-1
DOI 10.1007/978-3-540-85226-1 © 2008 Springer-Verlag Berlin Heidelberg This work is subject to copyright. All rights are reserved, whether the whole or part of the material is concerned, specifically the rights of translation, reprinting, reuse of illustrations, recitation, broadcasting, reproduction on microfilm or in any other way, and storage in data banks. Duplication of this publication or parts thereof is permitted only under the provisions of the German Copyright Law of September 9, 1965, in its current version, and permission for use must always be obtained from Springer. Violations are liable to prosecution under the German Copyright Law. The use of general descriptive names, registered names, trademarks, etc. in this publication does not imply, even in the absence of a specific statement, that such names are exempt from the relevant protective laws and regulations and therefore free for general use. Typesetting: digital data supplied by the authors Production: le-tex publishing services oHG, Leipzig, Germany Cover design: eStudioCalamar S.L., F. Steinen-Broo, Girona, Spain Printed on acid-free paper 987654321 springer.com
Preface Volume 2: Materials Science With the 14th European Microscopy Congress the European Microscopy Society (EMS), the German Society for Electron Microscopy (DGE) and the local organizers continue this successful series of conferences. Since the first congress in Stockholm in 1956 (still named European Congress on Electron Miscroscopy - EUREM), this conference series has become a well-accepted platform for academic and industrial scientists not only from Europe, but from all over the world, to discuss and exchange their latest results in the field of electron and other microscopies. The congress is subdivided into the three main areas, “Instrumentation and Methods”, “Materials Science” and “Life Sciences”. This 2nd volume of the conference proceedings collects the contributions related to the application of electron microscopy to the large field of Materials Science, again structured in five symposia covering all kinds of various materials: “Materials for Information Technology”, “Nanomaterials and Catalysts”, “Structural and Functional Materials”, “Soft Matters and Polymers”, and finally “Materials in Mineralogy, Geology and Archaeology”. All in all, this volume contains more than 400 contributions to this wide field of applications. Therefore, at this point we would like to express our deepest thanks to all, who contributed to making this a successful conference: the invited speakers and chairpersons, as well as all authors of contributed papers, may they be presented as oral communication or as poster. We are sure, that by the contributions of all of them the congress will reach an excellent level of scientific quality. Last, but not least, we want to thank all, who assisted in the organization of this conference, i.e. Tobias Caumanns, Achim Herwartz, Helga Maintz, Evi Münstermann, Daesung Park, Thomas Queck, Stefanie Stadler, Sarah Wentz, and especially the staffs of the Eurogress Conference Centre and of the Aachen Congress service. We wish all of you an exciting EMC2008! And after all the days of hard work, don’t forget to enjoy the marvellous city of Aachen. Silvia Richter and Alexander Schwedt Editors, Volume 2 of the EMC 2008 proceedings
Content M
Materials Science
Direct observation of atomic defects in carbon nanotubes and fullerenes ................ 1 K. Suenaga
Atomic studies on ferroelectric oxides by aberration corrected transmission electron microscopy........................................................................................................ 3 K. Urban and C.L. Jia
M1
Materials for Information Technology
M1.1 Si-based semiconductors Dark-field electron holography for the measurement of strain in nanostructures and devices ....................................................................................... 5 M.J. Hÿtch, F. Houdellier, F. Hüe, and E. Snoeck
Some device challenges towards the 22nm CMOS technology................................... 7 F. Andrieu, T. Ernst, O. Faynot, V. Delaye, D. Lafond, and S. Deleonibus
Off-axis electron holography for the analysis of nm-scale semiconductor devices. .............................................................................. 9 D. Cooper, R. Truche, L. Clement, S. Pokrant, and A. Chabli.
Influence of the oxide thickness................................................................................... 11 P. Donnadieu, V. Chamard, M. Maret, J.P. Simon, and P. Mur
Challenges to TEM in high performance microprocessor manufacturing.............. 13 H.J. Engelmann, H. Geisler, R. Huebner, P. Potapov, D. Utess, and E. Zschech
Strain study in transistors with SiC and SiGe source and drain by STEM nano beam diffraction................................................................................. 15 P. Favia, D. Klenov, G. Eneman, P. Verheyen, M. Bauer, D. Weeks, S.G. Thomas, and H. Bender
Cluster growth and luminescence in ion-implanted silica ........................................ 17 H.-J. Fitting, R. Salh, L. Kourkoutis, and B. Schmidt
Coherence Measurements of Bulk and Surface Plasmons in Semiconductors by Diffracted Beam Holography ................................................................................. 19 R.A. Herring
Comparison of 3D potential structures at different pn-junctions in FIB-prepared silicon and germanium samples measured by electron-holographic tomography ......................................................................... 21 A. Lenk, D. Wolf, H. Lichte, and U. Mühle
II
Content
EELS analyses of metal-inserted high-k dielectric stacks......................................... 23 M. MacKenzie, A.J. Craven, D.W. McComb, C.M. McGilvery, S. McFadzean, and S. De Gendt
Low voltage SEM observations of the dopant contrast in semiconductors ............. 25 K. Masenelli-Varlot, S. Luca, G. Thollet, P.H. Jouneau, and D. Mariolle
NiSi2/Si interface chemistry and epitaxial growth mode........................................... 27 S.B. Mi, C.L. Jia, K. Urban, Q.T. Zhao, and S. Mantl
Detailed investigation of a tunnel oxide defect in a flash memory cell using TEM-tomography............................................................................................... 29 U. Muehle, M. Krause, F. Goetze, D. Wolf, and U. Gaebler
Overgrowth of the Mn4Si7 phase on/around the hexagonal SiC and cubic MnSi impurity phases in the Mn4Si7/Si films............................................ 31 A. Orekhov, T. Kamilov, and E.I. Suvorova
HR-STEM EELS analysis of silicon 32 nm technology using a TITAN with a probe Cs corrector ............................................................................................ 33 R. Pantel, J.L Rouvière, E. Gautier, S. Denorme, C. Fenouiller-Beranger, F. Boeuf, G. Bidal, and M. Cheynet.
Tomographic analysis of a FinFET structure............................................................ 35 O. Richard, P. Van Marcke, and H. Bender
STEM EELS/EDX dopant analysis of nm-scale Si devices....................................... 37 G. Servanton, R. Pantel, M. Juhel, and F. Bertin
M1.2 Compound semiconductors Electron beam induced damage: An atom-by-atom investigation with TEAM0.5 .............................................................................................................. 39 C. Kisielowski, R. Erni, and J. Meyer
The atomic structure of GaN-based quantum wells and interfaces ......................... 41 C.J. Humphreys, M.J. Galtrey, R.A. Oliver, M.J. Kappers, D. Zhu, C. McAleese, N.K. van der Laak, D.M. Graham, P. Dawson, A Cerezo, and P.H. Clifton.
Using TEM to investigate antiphase disorder in GaP films grown on Si(001)........ 43 T.B. Adams, I. Nemeth, G. Lukin, B. Kunert, W. Stolz, and K. Volz
TEM characterization of InAs/GaAs quantum dots capped by a GaSb/GaAs layer.................................................................................................. 45 A.M. Beltrán, T. Ben, A.M. Sánchez, D.L. Sales, M.F. Chisholm, M. Varela, S.J. Pennycook, P.L. Galindo, J.M. Ripalda, and S.I. Molina
The microstructure of (0001)GaN films grown by molecular beam epitaxy from a nanocolumn precursor layer ........................................................................... 47 D. Cherns, L. Meshi, I. Griffiths, S. Khongphetsak, S.V. Novikov, N. Farley, R.P. Campion, and C.T. Foxon
Content
III
Compositional and Morphological Variation in GaN/AlN/AlGaN Heterostructures......................................................................... 49 P.D. Cherns, C. McAleese, M.J. Kappers, and C.J. Humphreys
TEM/STEM/EFTEM imaging and Valence Electrons Spectroscopy analysis of Ultra Low-K dielectrics ........................................................................................... 51 M. Cheynet, S. Pokrant, M. Aimadeddine, V. Arnal, and F. Volpi
Epitaxial Orientations of GaN Grown on R-plane Sapphire.................................... 53 J. Smalc-Koziorowska, G.P. Dimitrakopulos, Ph. Komninou, Th. Kehagias, S.-L. Sahonta, G. Tsiakatouras, and A. Georgakilas
Microstructure and growth model of MBE-grown InAlN thin films....................... 55 S.-L. Sahonta, A. Adikimenakis, G.P. Dimitrakopulos, Ph. Komninou, H. Kirmse, E. Pavlidou, E. Iliopoulos, A. Georgakilas, W. Neumann, and Th. Karakostas
Silicon carbide modulated structures as a result of the introduction of 8H bands in a 4H matrix ......................................................................................... 57 N. Frangis, M. Marinova, I. Tsiaoussis, E.K. Polychroniadis, T. Robert, S. Juillaguet, and J. Camassel
HRTEM study of AlN/3C-SiC heterointerfaces grown on Si(001) and Si(211) substrates .................................................................................................. 59 T. Isshiki, K. Nishio, Y. Abe, J. Komiyama, S. Suzuki, and H. Nakanishi
Electron microscopy of GaAs/AlGaAs quantum cascade laser................................ 61 A. Łaszcz, J. Ratajczak, A. Czerwinski, K. Kosiel, J. Kubacka-Traczyk, J. Muszalski, M. Bugajski, and J. Kątcki
Solving the crystal structure of highly disordered Sn3P4 by HRTEM ..................... 63 O.I. Lebedev, A.V. Olenev, and G. Van Tendeloo
Determination of In-distribution in InGaAs quantum dots...................................... 65 D. Litvinov, H. Blank, R. Schneider, D. Gerthsen, and M. Hetterich
Nanoanalytical investigation of the dielectric gate stack for the realisation of III-V MOSFET devices............................................................................................ 67 P. Longo, A.J. Craven, M.C. Holland, and I.G. Thayne
Phase mapping of uncapped InN quantum dots........................................................ 69 J.G. Lozano, M. Herrera, R. García, N.D. Browning, S. Ruffenach, O. Briot, and D. González
STEM investigations of (In,Ga)N/GaN quantum wells............................................. 71 P. Manolaki, I. Häusler, H. Kirmse, W. Neumann, P. Vennéguès, P. De Mierry, and P. Demolon
Defects in m-plane GaN layers grown on (100) γ-LiAlO2 ......................................... 73 A. Mogilatenko, W. Neumann, T. Wernicke, E. Richter, M. Weyers, B. Velickov, and R. Uecker
IV
Content
Improvements on InP epilayers by the use of monoatomic hydrogen during epitaxial growth and successive annealing ................................................................. 75 F.M. Morales, A. Aouni, R. García, P.A. Postigo, C.G. Fonstad, and S.I. Molina
Study of microstructure and strain relaxation on thin InXGa1-xN epilayers with medium and high In contents.............................................................................. 77 F.M. Morales, J.G. Lozano, R. García, V. Lebedev, S. Hauguth-Frank, V. Cimalla, O. Ambacher, and D. González
Convergence of microscopy techniques for nanoscale structural characterization: an illustration with the study of AlInN......................................... 79 A. Mouti, S. Hasanovic, M. Cantoni, E. Feltin, N. Grandjean, and P. Stadelmann
TEM analyses of microstructure and composition of AlxGa1-xN/GaN distributed Bragg reflectors ........................................................................................ 81 A. Pretorius, A. Rosenauer, T. Aschenbrenner, H. Dartsch, S. Figge, and D. Hommel
TEM study of quaternary InGaAsN/GaAs quantum well structures grown by molecular beam epitaxy.......................................................................................... 83 T. Remmele, M. Albrecht, I. Häusler, L. Geelhaar, H. Riechert, H. Abu-Farsakh, and J. Neugebauer
Lattice polarity and capping of GaN dots studied by Z-contrast imaging .............. 85 J.L. Rouviere, C. Bougerol, J. Coraux, B. Amstatt, E. Bellet-Amalric, and B. Daudin
Investigation of swift ions damage in wide band gap wurtzite semiconductors...... 87 S. Mansouri, I. Monnet, H. Lebius, G. Nouet, and P. Ruterana
A TEM analysis of the damage formation in thin GaN and AlN layers during rare earth ion implantation at medium range energy .................................. 89 F. Gloux, M.P Chauvat, and P. Ruterana
Characterization and modelling of semiconductor quantum nanostructures grown by droplet epitaxy ............................................................................................. 91 D.L. Sales, J.C. Hernandez, P.A. Midgley, A.M. Beltran, A.M. Sanchez, T. Ben, P. Alonso-González, Y. Gonzalez, L. Gonzalez, and S.I. Molina
Transmission Electron Microscopy Investigation of Self-Organized InN Nano-columns......................................................................... 93 H. Schuhmann, C. Denker, T. Niermann, J. Malindretos, A. Rizzi, and M. Seibt
Investigations on a dilute magnetic semicondutor (Ga1-xMnxAs) by conventional TEM and EELS ................................................................................ 95 M. Soda, U. Wurstbauer, M. Hirmer, W. Wegscheider, and J. Zweck
About the determination of optical properties using fast electrons ......................... 97 M. Stöger-Pollach
Content
V
M1.3 Data storage/ non-volatile memories Mapping uncompensated spins in exchange-biased systems by high resolution and quantitative magnetic force microscopy.............................. 99 H. J. Hug, M. Marioni, S. Romer, I. Schmid, and S. Romer
Ferroelectric materials and structures suitable for data storage: The role of microscopies in establishing preparation-microstructure-property relations ...................................................... 101 D. Hesse, M. Alexe, K. Boldyreva, H. Han, W. Lee, A. Lotnyk, B.J. Rodriguez, S. Senz, I. Vrejoiu, and N.D. Zakharov
Electronic structures at Magnetic Tunnel Junction interfaces: EELS experiments and FEFF calculations .............................................................. 103 K. March, D. Imhoff, G. Krill, and C. Colliex
Stability and reaction of magnetic sensor materials studied by atom probe tomography ....................................................................................... 105 G. Schmitz, C. Ene, H. Galinski, and V. Vovk
Transmission Electron Microscopy Analysis of Tunnel Magneto Resistance Elements with Amorphous CoFeB Electrodes and MgO Barrier .......................... 107 Michael Seibt, Gerrit Eilers, Marvin Walter, Kai Ubben, Karsten Thiel, Volker Drewello, Andy Thomas, Günter Reiss, and Markus Münzenberg
Study of the intermixing of Fe–Pt multilayers by analytical and high-resolution transmission electron microscopy........................................... 109 W. Sigle, T. Kaiser, D. Goll, N.H. Goo, V. Srot, P.A. van Aken, E. Detemple, and W. Jäger
Exploring structural dependence of magnetic properties in FePt nanoparticle by Cs-corrected HRTEM ....................................................... 111 Z.L. Zhang, J. Biskupek, U. Kaiser, U. Wiedwald, L. Han, and P. Ziemann
M1.4 Nanotubes, nanowires and molecular devices Understanding the Chemistry of Molecules in Nanotubes by Transmission Electron Microscopy .................................................................................................. 113 A.N. Khlobystov, M.W. Fay, and P.D. Brown
Electrical and mechanical property studies on individual low-dimensional inorganic nanostructures in HRTEM....................................................................... 115 D. Golberg, P.M.F.J. Costa, M. Mitome, Y. Bando, and X.D. Bai
Atomic structure of SW-CNTs: correlation with their growth mechanism and other electron diffraction studies....................................................................... 117 R. Arenal, M.F. Fiawoo, R. Fleurier, M. Picher, V. Jourdain, A.M. Bonnot, and A. Loiseau
VI
Content
TEM investigation ofSe nanostructures in/on Acetobacter xylinum cellulose gel-film ......................................................................................................... 119 N. Arkharova, V.V. Klechkovskaya, and E. Suvorova
In-situ electron irradiation studies of metal-carbon nanostructures ..................... 121 L. Sun, Y. Gan, J.A. Rodriguez-Manzo, M. Terrones, A.V. Krasheninnikov, and F. Banhart
Application of 80kV Cs-corrected TEM for nanocarbon materials ...................... 123 A. Chuvilin, U. Kaiser, D. Obergfell, A. Khlobystov, and S. Roth
Control of gold surface diffusion on Si nanowires................................................... 125 M.I. den Hertog, J.-L. Rouviere, F. Dhalluin, P.J. Desré, P. Gentile, P. Ferret, F. Oehler, and T. Baron
Nanowires of Semiconducting Metal-oxides and their Functional Properties...... 127 M. Ferroni, C. Baratto, E. Comini, G. Faglia, L. Ortolani, V. Morandi, S. Todros, A. Vomiero, and G. Sberveglieri
Phase relations in the Fe–Bi–O system under hydrothermal conditions............... 129 A. Gajović, S. Šturm, B. Jančar, and M. Čeh
Dose dependent crystallographic structure of InAs nanowires.............................. 131 F. Gramm, E. Müller, I. Shorubalko, R. Leturcq, A. Pfund, R. Wepf, and K. Ensslin
HRTEM simulations of planar defects in ZnTe nanowires .................................... 133 I. Häusler, H. Kirmse, W. Neumann, S. Kret, P. Dłużewski, E. Janik, G. Kraczewski, and T. Wojtowicz
A universal method for determination of helicities present in unidirectional groupings of graphitic or graphitic-like tubular structures ................................... 135 H. Jiang, D.P. Brown, A.G. Nasibulin, and E.I. Kauppinen
Microstructure of (112) GaAs nanorods grown by MBE ....................................... 137 E. Johnson, S.A. Jensen, L.P. Hansen, C.B. Sørensen, and J. Nygård
Structural characterization of ZnO nanorods grown on sapphire substrate by MOCVD ................................................................................................................. 139 P.-H. Jouneau, M. Rosina, G. Perillat, P. Ferret, and G. Feuillet
Nucleation of Metal Clusters on Carbon Nanotubes............................................... 141 X. Ke, A. Felten, D. Liang, S. Bals, J.J. Pireaux, J. Ghijsen, W. Drube, M. Hecq, C. Bittencourt, and G. Van Tendeloo
EDX and linescan modelling for core/shell GaN/AlGaN nanowire analysis ......... 143 L. Lari, R.T. Murray, T. Bullough, P.R. Chalker, C. Chèze, L. Geelhaar, and H. Riechert
Mo6S9-xIx nanowires: structure studies by aberration corrected high resolution TEM and STEM ....................................................................................... 145 V. Nicolosi, J.N. Coleman, D. Mihailovic, and P. Nellist
Discrete Atom Imaging in Carbon Nanotubes and Peapods Using Cs-Corrected TEM Operated at 100keV.................................................................. 147 Luca Ortolani, Florent Houdellier, and Marc Monthioux
Content
VII
Extended Defects in Semiconductor Nanowires ...................................................... 149 Peter Pongratz, Youn-Joo Hyun, Alois Lugstein, Aaron Andrews, and Emmerich Bertagnolli
Surface chemistry along a single silicon nanowire: Quantitative x-ray photoelectron emission microscopy (XPEEM) of the metal catalyst diffusion ..... 151 O. Renault, A. Bailly, P. Gentile, N. Pauc, T. Baron, L.–F. Zagonel, and N. Barrett
TEM characterization of metallic Ni nanoshells grown on gold nanorods and on carbon nanotubes........................................................................................... 153 J.B. Rodríguez-González, M. Grzelczak, M.A. Correa-Duarte, J. Pérez-Juste, and L.M. Liz-Marzán
Electron Irradiation Effects in Carbon Nanostructures: Surface Reconstruction, Extreme Compression, Nanotube Growth and Morphology Manipulation ................................................................................. 155 M. Terrones, L. Sun, J.A. Rodriguez-Manzo, H. Terrones, and F. Banhart
Crystallographic phase and orientation analysis of GaAs nanowires by ESEM, EDS, TEM, HRTEM and SAED............................................................. 157 A.M. Tonejc, S. Gradečak, A. Tonejc, M. Bijelić, H. Posilović,V. Bermanec, and M. Tambe
3-Dimensional Morphology of GaP-GaAs nanowires ............................................. 159 M.A. Verheijen, R. Algra,M.T. Borgström, G. Immink, E. Sourty, L.F. Feiner, W.J.P. van Enckevort, E. Vlieg, and E.P.A.M. Bakkers
Characteristics of Indium-Catalyzed Si Nanowires ................................................ 161 Z.W. Wang, Z.Y. Li, and F. Iacopi
M2
Nanomaterials and Catalysts
M2.1 Carbon-based HRTEM contribution to the study of extraterrestrial nanocarbons and some earth materials analogues ......................................................................... 163 J.N. Rouzaud and C. Le Guillou
Time resolved in-situ TEM observations of Carbon Nanotube growth................. 165 J. Robertson, S. Hofmann, R. Sharma, C. Ducati, and R. Dunin-Borkowski
Insulator-Metal transition: formation of Diamond Nanowires in n-type Conductive UNCD films ............................................................................ 167 R. Arenal, O. Stephan, P. Bruno, and D.M. Gruen
Field emission from iron-filled carbon nanotubes observed in-situ in the scanning electron microscope ......................................................................... 169 K.J. Briston, Y. Peng, N. Grobert, A.G. Cullis, and B.J. Inkson
Templated ordering of fullerenes on nanostructured oxide surfaces .................... 171 D.S. Deak, B.C. Russell, D.T. Newell, K. Porfyrakis, F. Silly, and M.R. Castell
VIII
Content
Carbon nanostructures produced by chlorination of Cr3C2 and Cr(acac)3 .......... 173 A. Gómez-Herrero, E. Urones-Garrote, D. Ávila-Brande, N.A. Katcho, E. Lomba, A.R. Landa-Cánovas, and L.C. Otero-Díaz
Structural peculiarities of carbon onions, formed by different methods .............. 175 B.A. Kulnitskiy, I.A. Perezhogin, and V.D. Blank
Electron Energy Loss Spectroscopy of La@C82 peapods........................................ 177 R.J. Nicholls, D.A. Eustace, D. McComb, G.A.D. Briggs, D.J.H. Cockayne, and D.G. Pettifor
HRTEM studies of Y-junction bamboo-like CN-nanotubes................................... 179 I.A. Perezhogin, B.A. Kulnitskiy, V.D. Blank, D.V. Batov, and E.V. Polyakov
EF-TEM observation of biological tissue for risk assessment of fullerene nanoparticles .......................................................................................... 181 K. Yamamoto, M. Makino, E. Kobayashi, and Y. Morimoto
M2.2 Nanoparticles and catalysts Looking at the surface of catalysts nanopowders .................................................... 183 J.C. Hernandez, A.B. Hungria, M. Lopez-Haro, J.A. Perez-Omil, S. Trasobares, S. Bernal, P. Midgley, O. Stephan, and J.J. Calvino
Gathering structural and analytical information on catalysts at sub-nanometer level with TEM............................................................................. 185 F.J. Cadete Santos Aires and M. Aouine
Size effect and influence of nanoparticles thickness on order/disorder phenomena in CoPt nanoparticles ............................................. 187 D. Alloyeau, C. Ricolleau, T. Oikawa, C. Langlois, Y. Le Bouar, and A. Loiseau
In situ L10 ordering of FePt nanoparticles ............................................................... 189 P. Bayle-Guillemaud, M. Delalande, V. Monnier, Y. Samson, and P. Reiss
Characterization of indium doped zinc oxide nanorods ......................................... 191 H. Burghardt, H. Schmid, and W. Mader
Adsorbate-induced restructuring on Pt nanoparticles studied by environmental transmission electron microscopy .............................................. 193 M. Cabié, S. Giorgio, and C.R. Henry
EELS in monochromated and Cs probe corrected TEM: ...................................... 195 M. Cheynet, S. Pokrant, and S. Ersen.
Atomic-resolution Electron Microscopy at Ambient Pressure............................... 197 J.F. Creemer, S. Helveg, A.M. Molenbroek, P.M. Sarro, and H.W. Zandbergen
Development of a system for TEM/STEM investigation of air-sensitive materials: Preliminary results on CeO2 reduction behaviour ................................ 199
J.J. Delgado, M. López-Haro, J.D. López-Castro, J.A. Pérez-Omil, S. Trasobares, and J.J. Calvino
Content
IX
Characterization of two new zeolites by combining Electron Microscopy and X-Ray Powder Diffraction analyses .................................................................. 201 E. Di Paola, E. Montanari, S. Zanardi, and A. Carati
Electron beam-induced effects on copper nanoparticles: coarsening and generation of twins........................................................................... 203 D. Díaz-Droguett, V. Fuenzalida, and G. Solórzano
Role of the catalyst and substrate in nucleation and growth of Single Wall Carbon Nanotubes in HFCVD ......................................................... 205 M.-F. Fiawoo, N. Brun, A.-M Bonnot, O. Stephan, J. Thibaultand, and A. Loiseau
PEMFC degradation phenomena studied by electron microscopy........................ 207 L. Guetaz, B. Vion-Dury, and S. Escribano
TEM investigation of magnetite nanoparticles for biomedical applications ......... 209 S. Gustafsson, A. Fornara, F. Ye, K. Petersson, C. Johansson, M. Muhammed, and E. Olsson
Catalytic soot oxidation studied by Environmental Transmission Electron Microscopy .................................................................................................. 211 S.B. Simonsen, S. Dahl, E. Johnson, and S. Helveg
Surface and interface structure of ceria supported ruthenium.............................. 213 J.C. Hernandez, S. Trasobares, J.M. Gatica, D.M. Vidal,M.A. Cauqui, J.J. Calvino, A.B. Hungria, and J.A. Perez-Omil
Characterisation of materials with applications in the photocatalytic activation of water .................................................................. 215 N.S. Hondow, R. Brydson, Y.H. Chou, and R.E. Douthwaite
Complementary EM study on highly active nanodendritic Raney-type Ni catalysts with hierarchical build-up.......................................................................... 217 U. Hörmann, U. Kaiser, N. Adkins, R. Wunderlich, A. Minkow, H. Fecht, H. Schils, T. Scherer, and H. Blumtritt
Structural properties of sol-gel synthesized Li+-doped titania nanowhisker arrays.................................................................................................... 219 U. Hörmann, J. Geserick, S. Selve, U. Kaiser, and N. Hüsing
Quantitative strain determination in nanoparticles using aberration-corrected HREM........................................................................... 221 C.L. Johnson, E. Snoeck, M. Ezcurdia, B. Rodríguez-González, I. Pastoriza-Santos, L.M. Liz-Marzán, and M.J. Hÿtch
Morphological characterization by HRTEM and STEM of Fe3O4 hollow nano-spheres.................................................................................... 223 A. Ibarra, G.F. Goya, J. Arbiol, E. Jr. Lima, H. Rechenberg, J. Vargas, R. Zysler, and M.R. Ibarra
Direct observation of surface oxidation of Rh nanoparticles on (001) MgO......... 225 N.Y. Jin-Phillipp, P. Nolte, A. Stierle, P.A. van Aken, and H. Dosch
X
Content
Characterization of catalyst poisoning in biodiesel and conventional diesel fuelled vehicles ................................................................... 227 T. Kanerva, K. Kallinen, Toni Kinnunen, M. Vippola, and T. Lepistö
TEM Characterisation of Highly Luminescent CdS Nanocrystals ........................ 229 H. Katz, A. Izgorodin, D.R. MacFarlane, and J. Etheridge
Structure and composition of dilute Co-doped BaTiO3 nanoparticles .................. 231 O.I. Lebedev, R. Erni, and G. Van Tendeloo
CoxFe3-xO4 catalytic materials for gaz sensors ......................................................... 233 L. Ajroudi, A. Essoumhi, S. Villain, V. Madigou, N. Mliki, and Ch. Leroux
(S)TEM investigation on the role of alumina dopants to prevent redox activity decay at high temperature in CePrOx /doped-Al2O3 catalysts .................. 235 M. López-Haro, K. Aboussaid, J.M. Pintado, J.J. Calvino, and S. Trasobares
Sulfated Zirconia Catalysts: Structure and Performance Relationship, a TEM Study............................................................................................................... 237 C. Meyer, D. Su, N. Hensel, F.C. Jentoft, and R. Schlögl
A novel procedure for an accurate estimation of the lattice parameter of supported metal nanoparticles from the analysis of plan view HREM images ....................................................................................... 239 C. Mira, J.A. Perez-Omil, J.J. Calvino, and S. Bernal
Microstructure of Pt particles and aggregates deposited on different carbon materials for fuel cells application ............................................................................ 241 D. Mirabile Gattia, E. Piscopiello, M. Vittori Antisari, S. Bellitto, S. Licoccia, E. Traversa, L. Giorgi, R. Marazzi, and A. Montone
Low-loss-energy EFTEM imaging of triangular silver nanoparticles ................... 243 J. Nelayah, L. Gu, W. Sigle, C.T. Koch, L. Pastoriza-Santos, L.M. Liz-Marzan, and P.A. van Aken
Microstructure of cobalt nanocluster arrays fabricated by solid-state dewetting.............................................................................................. 245 Y.-J. Oh, J. Kim, S. Hwang, C.A. Ross, and C.V. Thompson
Size Effect in Gold Nanoparticles Investigated by Electron Holography and STEM ................................................................................................................... 247 L. Ortolani, V. Morandi, and M. Ferroni
Post-Mortem investigation of Fischer Tropsch catalysts using cryo- transmission electron microscopy ......................................................... 249 D. Ozkaya, M. Lok, J. Casci, and P. Ash
TEM Investigations on Cu-impregnated Zeolite Y catalysts via chloride free preparation..................................................................................... 251 M.-M. Pohl, M. Richter, and M. Schneider
Content
XI
Coarsening of mass-selected Au clusters on amorphous carbon at room temperature .................................................................................................. 253 R. Popescu, R. Schneider, D. Gerthsen, A. Böttcher, D. Löffler, and P. Weiss
TEM investigations on Ni clusters electrodeposited on Carbon substrate............ 255 M. Re, M.F. De Riccardis, D. Carbone, D. Wall, and M. Vittori Antisari
Near-surface structure of FePt nanoparticles.......................................................... 257 B. Rellinghaus, D. Pohl, E. Mohn, and L. Schultz
Overgrowth of gold nanorods: From rods to octahedrons ..................................... 259 J.B. Rodríguez-González, E. Carbó-Argibay, I. Pastoriza-Santos, J. Pérez-Juste, and L.M. Liz-Marzán
Reactive Diffusion under Laplace Tension in Spherical Nanostructures.............. 261 C. Ene, C. Nowak, and G. Schmitz
Preparation and characterization of palladium nanoparticles with various size distributions................................................................................... 263 M. Slouf, H. Vlkova, and D. Kralova
Electron microscopy for the characterization of nanoparticles ............................. 265 D. Sommer and U. Golla-Schindler
Titanium dioxide nanoparticles prepared from TiOSO4 aqueous solutions ......... 267 J. Šubrt, J. Boháček, N. Murafa, and L. Szatmáry
Exploring nanoscale ferroelectricity in isolated and interacting colloidal ferroelectric nanocrystals using electron holography ............................................. 269 D. Szwarcman, Y. Lereah, G. Markovich, M. Linck, and H. Lichte
STEM investigation on the one-pot synthesis of nanostructured CexZr1-xO2-BaO·nAl2O3 catalytic materials ............................................................. 271 J.C. Hernandez, J.A. Perez-Omil, J.J. Calvino, S. Bernal, R. di Monte, S. Desinan, J. Kašpar, and S. Trasobares
Enhanced stability against oxidation due to 2D self-organisation of hcp cobalt nanocrystals ......................................................................................... 273 Isabelle Lisiecki, S. Turner, S. Bals, M.P. Pileni, and G. Van Tendeloo
Loaded porous Zn4O(bdc)3 (metal@MOF-5) frameworks characterised by TEM ....................................................................................................................... 275 S. Turner, O.I. Lebedev, F. Schröder, R.A. Fischer, and G. Van Tendeloo
Growth behaviour of sub-nm sized focused electron beam induced deposits ....... 277 W.F. van Dorp, C.W. Hagen, P.A. Crozier, P. Kruit, S. Zalkind, B. Yakshinskiy, and T.E. Madey
Ruthenium deposition on CO2-treated and untreated carbon black investigated by electron tomography........................................................................ 279 M. Wollgarten, R. Grothausmann, P. Bogdanoff, G. Zehl, I. Dorbandt, S. Fiechter, and J. Banhart
XII
Content
Size-dependent crystallinity and relative orientations of nano-Pt/γ-Al2O3 ............ 281 J.C. Yang, L. Li, S. Sanchez, J.H. Kong, Q. Wang, L.L. Wang, Z. Zhang, D.D. Johnson, A.I. Frenkel, and R.J. Nuzzo
Formation of nanometer-sized porous GaSb particles by vacancy clustering induced by electronic excitation ................................................................................ 283 H. Yasuda, A. Tanaka, N. Nitta, K. Matsumoto, and H. Mori
Structural investigations of membrane electrode assemblies in fuel cells via environmental scanning electron microscopy.................................................... 285 S. Zils, N. Benker, and C. Roth
M2.3 Nanostructured materials and Nanolab In situ TEM nanocompression testing ...................................................................... 287 A.M. Minor, J. Ye, and R.K. Mishra
Physical measurements on an individual nanostructure in a TEM nanolaboratory.......................................................................................... 289 M. Kobylko, S. Mazzucco, R. Bernard, M. Kociak, and C. Colliex
TEM study of nanostructured BZO templates in (001)-LAO and (001)-STO substrates for the growth of superconducting YBCO films.................................... 291 P. Abellan, M. Gibert, F. Sandiumenge, M.J. Casanove, T. Puig, and X. Obradors
Hydrothermal synthesis and characterisation of single crystal α-Fe2O3 nanorods ....................................................................................................... 293 T. Almeida, Y.Q. Zhu, and P.D. Brown
GaAs NWs and Related Quantum Heterostructures Grown by Ga-Assisted Molecular Beam Epitaxy: Structural and Analytical Characterization................ 295 J. Arbiol, S. Estradé, F. Peiró, J.R. Morante, C. Colombo, D. Spirkoska, G. Abstreiter, and A. Fontcuberta i Morral
A method for in-situ electrical measurements of thin film heterostructures using TEM and SEM.................................................................................................. 297 J. Börjesson, A. Kalabukhov, K. Svensson, and E. Olsson
Electron Beam Nanofabrication and Characterization of Iron Compounds ........ 299 K. Furuya, M. Shimojo, M. Takeguchi, M. Song, K. Mitsuishi, and M. Tanaka
TEM analysis of the chemical gradient in (Zn,Mn)Te/ZnTe nanowires .............. 301 H. Kirmse, W. Neumann, S. Kret, P. Dłużewski, E. Janik, W. Zaleszczyk, A. Presz, G. Karczewski, and T. Wojtowicz
Structural and morphological characterization of GaN/AlGaN quantum dots by transmission electron microscopy........................................................................ 303 M. Korytov, M. Benaissa, J. Brault, T. Huault, and P. Vennéguès
Structure and stability of core-shell AuAg nanopartciels....................................... 305 Z.Y. Li, R. Merrifield, Y. Feng, J.P. Wilcoxon, R.E. Palmer, A.L. Bleloch, M. Gass, and K. Sader
Content
XIII
In-situ studies on electrical and mass transport in multi-wall carbon and vanadium oxide nanotubes................................................................................. 307 M. Löffler, T. Gemming, R. Klingeler, and B. Büchner
Electron microscopy of nano-magnesium produced by Inert Gas Condensation for hydrogen storage ................................................... 309 E. Piscopiello, E. Bonetti, E. Callini, L. Pasquini, and M. Vittori Antisari
Two Different Structures of Crystalline Mesoporous Indium Oxide Obtained by Nanocasting Process.............................................................................................. 311 E. Rossinyol, E. Pellicer, M. Cabo, O. Castell, and M.D. Baro
Measuring electrical properties of carbon nanotubes using liquid metal immersion, an in situ scanning electron microscopy study..................................... 313 H. Strand, K. Svensson, and E. Olsson
TEM characterization of biogenic metal nanoparticles .......................................... 315 E.I. Suvorova, P.A. Buffat, H. Veeramani, J. Sharp, E. Schofield, J. Bargar, and R. Bernier-Latmani
On the structure of VxOy supported on multiwalled carbon nanotubes................ 317 D. Wang, J.-P. Tessonnier, M. Willinger, C. Hess, D.S. Su, and R. Schlögl
Hexahedral nano-cementites catalysing the growth of carbon nanohelices .......... 319 J.H. Xia, X. Jiang, C.L. Jia, and C. Dong
M2.4 Thin films and interfaces Investigation of organic/inorganic interfaces using nano-analytical transmission electron microscopy ............................................................................. 321 V. Jantou, M.A. Horton, and D.W. McComb
Cationic ordering and interface effects in superlattices and nanostructured materials ................................................................................... 323 P. Boullay, W.C. Sheets, W. Prellier, E.-L. Rautama, A.K. Kundu, V. Caignaert, B. Mercey, and B. Raveau
Strain in SrTiO3 layers embedded in a scandate/titanate multilayer system........ 325 D. Ávila, M. Boese, T. Heeg, J. Schubert, and M. Luysberg
Anisotropic growth of CGO islands on the (001)-LaAlO3 surface ........................ 327 A. Benedetti, M. Gibert, F. Sandiumenge, T. Puig, and X. Obradors
Diffraction contrast imaging and high resolution transmission electron microscopy of multiferroic thin films and heterostructures................................... 329 B.I. Birajdar, I. Vrejoiu, X.S. Gao, B.J. Rodriguez, M. Alexe, and D. Hesse
Imaging of compositional defects at silicide-silicon interfaces using aberration corrected HAADF ...................................................................................................... 331 M. Falke, U. Falke, P. Wang, and A. Bleloch
XIV
Content
Characterization of nanometric oxide particles extracted from a steel surface onto a carbon replica ............................................................... 333 P. Haghi-Ashtiani, A. Ollivier, and M.-L. Giorgi
TEM characterization of textured silicon heterojunction solar cells..................... 335 A. Hessler-Wyser, C. Monachon, S. Olibet, and C. Ballif
Investigation of the change in the microstructure of thin p-type Bi-Sb-Te thermoelectric films after heat treatment ................................................................ 337 F. Heyroth, M. Schade, K. Rothe, H.S. Leipner, and M. Stordeur
EM study on forming Inorganic film with Periodically Organized Mesopores upon Polymer film...................................................................................................... 339 H. Wenqing, Z. Ying, Y. Fang, Zhaoxi, and Y. Wantai
Nanointerface analysis of hard coatings deposited by IBAD.................................. 341 D. Kakas, B. Skoric, A. Miletic, and L. Kovacevic
Transrotational crystals growing in amorphous Cu-Te film.................................. 343 V.Yu. Kolosov, A.V. Kozhin, L.M. Veretennikov, and C.L. Schwamm
TEM investigation of sputtered indium oxide layers on silicon substrate for gas sensors............................................................................................................. 345 Th. Kups, I. Hotovy, and L. Spieß
Microstructure of Sr4Ru2O9 thin films and Bi3.25La0.75Ti3O12/Sr4Ru2O9 bilayers................................................................... 347 R. Chmielowski, V. Madigou, M. Blicharski, and Ch. Leroux
Analysis of the LSM/YSZ interface on micro- and nano-scale by SEM, FIB/SEM and (S)TEM ............................................................................................... 349 Y. Liu, L. Theil Kuhn, and J.R. Bowen
ESI and HRTEM of chemical solution deposited (CSD) ........................................ 351 L. Molina, T. Thersleff, B. Rellinghaus, B. Holzapfel, and O. Eibl
CTEM diffraction contrast of biaxially-textured La2Zr2O7 buffer layers on nickel substrates .................................................................................................... 353 L. Molina, S. Engel, B. Holzapfel, and O. Eibl
TEM sample preparation of YBCO-coated conductors: conventional method and FIB........................................................................................................................ 355 L. Molina, T. Thersleff, C. Mickel, S. Menzel, B. Holzapfel, and O. Eibl
Nucleation and evolution of biepitaxial YBa2Cu3O7-δ thin film grown on SrTiO3 and MgO substrates ................................................................................. 357 H. Pettersson, K. Cedergren, D. Gustafsson, R. Ciancio, F. Lombardi, and E. Olsson
An investigation of Al-Pb interfaces using probe-corrected high-resolution STEM................................................................................................ 359 H. Rösner, S. Lopatin, B. Freitag, and G. Wilde
Content
XV
Spectrometric Full-Color Cathodoluminescence Electron Microscopy Study of Grain Boundaries of ZnO Varistor ...................................................................... 361 H. Saijo, N. Daneu, A. Recnik, and M. Shiojiri
Study of structural properties of Mo/CuInS2/ZnS used in solar cells by TEM..... 363 J. Sandino, G. Gordillo, and H. Lichte
Texture analysis of silicide thin films: combining statistical and microscopical information.................................................................................. 365 H. Schletter, S. Schulze, M. Hietschold, K. De Keyser, C. Detavernier, G. Beddies, A. Bleloch, and M. Falke
Statistical Tomography of 3D Thin Film Structure using Transmission Electron Microscopy .................................................................................................. 367 E. Spiecker, V. Radmilovic, and U. Dahmen
Analytical TEM investigations of Pt/YSZ interfaces............................................... 369 V. Srot, M. Watanabe, C. Scheu, P.A. van Aken, E. Mutoro, J. Janek, and M. Rühle
Microstructure and self-organization of nano-engineered artificial pinning centers in YBa2Cu3O7-x coated conductors................................................. 371 T. Thersleff, E. Backen, S. Engel, C. Mickel, L. Molina-Luna, O. Eibl, B. Rellinghaus, L. Schultz, and B. Holzapfel
The determination of the interface structure between ionocovalent compounds: the general case study of the Al2O3-ZrO2 large misfit system........... 373 G. Trolliard, and D. Mercurio
Simple method to improve quantification accuracy of energy-dispersive X-ray spectroscopy in an analytical transmission electron microscope by specimen tilting...................................................................................................... 375 T. Walther
Comparison of transmission electron microscopy methods to measure layer thicknesses to sub-monolayer precision.................................................................... 377 T. Walther
Determination of interface structure of YBCO/LCMO by a spherical aberration- corrected HRTEM......................................................... 379 Z.L. Zhang, U. Kaiser, S. Soltan, and H.-U. Habermeier
HREM characterization of BST-MgO interface...................................................... 381 O.M. Zhigalina, A.N. Kuskova, A.L. Chuvilin, V.M. Mukhortov, Yu.I. Golovko, and U. Kaiser
M3
Structural and Functional Materials
M3.1 Alloys and Intermetallics TEM investigations on novel shape memory systems with Ni-depletions ............. 383 D. Schryvers, R. Delville, B. Bartova, and H. Tian
XVI
Content
Crystalline-to-amorphous transformation in intermetallic compounds by severe plastic deformation .................................................................................... 385 K. Tsuchiya, T. Waitz, T. Hara, H.P. Karnthaler, Y. Todaka, and M. Umemoto
EELS quantification of complex nitrides in a 12 % Cr steel .................................. 387 M. Albu, F. Méndez Martin, and G. Kothleitner
Formation of ordered solid solution during phase separation in Cu-Ag alloy films.................................................................................................... 389 F. Misják, P.B. Barna, and G. Radnóczi
Precipitates and magnetic domains in an annealed Co38Ni33Al29 shape memory alloy studied by TEM................................................................................................. 391 B. Bartova, D. Schryvers, N. Wiese, and J.N. Chapman
On the gallium accumulation at the boundaries of Al layers in FIB prepared TEM specimens.......................................................................................... 393 P. Favia and H. Bender
Precipitation in an Al-Mg-Ge Alloy.......................................................................... 395 R. Bjorge, C.D. Marioara, S.J. Andersen, and R. Holmestad
Interaction between dislocations and oxide precipitates in an aluminium containing ferritic stainless steel ............................................................................... 397 L. Boulanger, S. Poissonnet, and F. Legendre
Voids Associated with Nano-Particles of Tin in Aluminium .................................. 399 L. Bourgeois, M. Weyland, and B.C. Muddle
Influence of thermal treatments in microstructure and recrystallization peak energy of P/M Al-Mg-X alloys................................................................................... 401 S.J. Buso, A. Almeida Filho, I.M. Espósito, J.R. Matos, and W.A. Monteiro
Analytical TEM of Nb3Sn Multifilament Superconductor Wires .......................... 403 M. Cantoni, V. Abächerli, D. Uglietti, B. Seeber, and R. Flükiger
3D Reconstruction of Ni4Ti3 Precipitates in Ni-Ti by FIB/SEM Slice-and-View...................................................................................... 405 S. Cao, W. Tirry, W. Van Den Broek, and D. Schryvers
Electron microscopy study of Mg78.5Pd21.5: aphase with nanothin 120° rotational twin domains..................................................................................... 407 W. Carrillo-Cabrera, J.P.A. Makongo, Yu. Prots, and G. Kreiner
Analysing small precipitates in a ferritic steel matrix............................................. 409 A.J. Craven and M. MacKenzie
Failure analysis of first stage land-based gas turbine blades.................................. 411 F. Delabrouille, F. Arnoldi, L. Legras, and C. Cossange
TEM investigation of microstructures in low-hysteresis Ti50Ni50-xPdx alloys with special lattice parameters .................................................................................. 413 R. Delville, D. Schryvers, Z. Zhang, S. Kasinathan, and R.D. James
Content
XVII
Evidence of silica layer at the interface between ferrite and the chromium oxide scale in oxidized Fe-Cr-Si alloys ..................................... 415 G. Bamba, P. Donnadieu, Y. Wouters, and A. Galerie
Applying a classical 2 beam diffraction contrast method for measuring nanoprecipitate misfit ....................................................................... 417 L. Lae and P. Donnadieu
Microstructure and interface composition of γ-phase in Co38Ni33Al29 shape memory alloy.......................................................................... 419 R. Espinoza, B. Bartova, D. Schryvers, S. Ignacova, and P. Sittner
Microstructural characterization of the aluminum alloy 6063 after work hardening treatments .............................................................................. 421 I.M. Espósito, S.J. Buso, and W.A. Monteiro
Microstructure- mechanical property relationships in dual phase automotive strip steels................................................................................................ 423 V. Tzormpatzdi and G. Fourlaris
Electron diffraction analysis of nanocrystalline Fe-Al............................................ 425 C. Gammer, C. Mangler, C. Rentenberger, and H.P. Karnthaler
Dual Beam and TEM characterisation of deformation structures in fatigued austenitic stainless steel........................................................................... 427 A. Garcia, L. Legras, M. Akamatsu, and Y. Bréchet
Microstructural characterisation of steel heat-treated by the novel quenching and partitioning process .................................................... 429 K. He, D.V. Edmonds, J.G. Speer, D.K. Matlock, and F.C. Rizzo
Martensite tempering behaviour relevant to the quenching and partitioning process ............................................................................................ 431 K. He, D.V. Edmonds, J.G. Speer, D.K. Matlock, and F.C. Rizzo
Chemical and structural analysis of NiAl-Al2O3 interface by FETEM and STEM ................................................................................................................... 433 W. Hu, T. Weirich, and G. Gottstein
TEM investigations of aluminum precipitate in eutectic Si of A356 based alloys ................................................................................................... 435 Z.H. Jia, L. Arnberg, P. Åsholt, B. Barlas, and T. Iveland
Microstructure of slow-cooled wedge-cast Cu58Co42 alloy with a metastable liquid miscibility gap ................................................................... 437 E. Johnson, S. Curiotto, N. Pryds, and L. Battezzati
TEM investigations of Elektron 21 magnesium alloy after long-term annealing .......................................................................................... 439 A. Kielbus
Microstructure of AJ62 magnesium alloy after long-term annealing.................... 441 A. Kielbus and J. Mizera
XVIII
Content
EELS characterisation of the interface between nanoscaled ODS particles and matrix in advanced fusion steels ........................................................................ 443 M. Klimenkov, R. Lindau, and A. Möslang
Microstructure-mechanical property relationships in a maraging 250 steel ........ 445 P. Kokkonidis, E. Papadopoulou, A. Rizos, T. Koutsoukis, and G. Fourlaris
Microstructure of Co-Ni based superalloys ............................................................. 447 T.J. Konno, T. Tadano, H. Matsumoto, and A. Chiba
Precipitation reactions in superferritic stainless steels ........................................... 449 T. Koutsoukis, K. Konstantinidis, P. Kokkonidis, E. Papadopoulou, and G. Fourlaris
Effect of ageing in cold rolled superaustenitic stainless steels ................................ 451 S. Zormalia, T. Koutsoukis, E. Papadopoulou, P. Kokkonidis, and G. Fourlaris
Structure and properties of P/M material of AlMg – SiO2 system processed by mechanical alloying............................................................................................... 453 A. Kula, L. Błaż, M. Sugamata, J. Kaneko, Ł. Górka, J. Sobota, and G. Włoch
Extrusion of rapidly solidified 6061 + 26 wt% Si alloy ........................................... 455 A. Kula, M. Sugamata, J. Kaneko, L. Błaż, G. Włoch, J. Sobota, and W. Bochniak
TEM and EELS study of carbide precipitation in low alloyed steels..................... 457 C. Leguen, M. Perez, T. Epicier, D. Acevedo, and T. Sourmail
Microstructural analysis of plastically deformed complex metallic alloy κ-AlMnNi ........................................................................................................... 459 M. Lipińska-Chwałek, M. Heggen, M. Feuerbacher, and A. Czyrska-Filemonowicz
Electron microscopy analysis of Mn partitioning in retained austenitemartensite- bainite islands......................................................................................... 461 A. Lis, J. Lis, and P. Wieczorek
TEM characterization of microstructures in a Ni2MnGa alloy.............................. 463 H. Maeda, E. Taguchi, K. Inoue, and A. Sugiyama
Nanocrystalline FeAl produced by high pressure torsion studied by TEM in 3D ............................................................................................................. 465 C. Mangler, C. Rentenberger, and H.P. Karnthaler
HRTEM study of precipitates in Al-Mg-Si-(Ag, Cu) alloys.................................... 467 K. Matsuda, J. Nakamura, T. Kawabata, T. Sato, and S. Ikeno
Martensite structure of non-stoichiometric Co2NiGa ferromagnetic shape memory alloy .............................................................................................................. 469 K. Prusik and M. Morawiec
Electron microscopy of Fe and FeB atomic clusters in the Fe-based amorphous alloys structure ............................................................ 471 E.V. Pustovalov, V.S. Plotnikov, B.N. Grudin, S.V. Dolzhikov, E.B. Modin, O.V. Voitenko, and E.S. Slabzhennikov
Content
XIX
Core/Shell Precipitates in Al-Li-Sc-Zr Alloys.......................................................... 473 V. Radmilovic, M.D. Rossell, A. Tolley, E.A. Marquis, R. Erni, and U. Dahmen
Analysis of basic mechanisms of hardening in ODS EUROFER97 steel using in-situ TEM ....................................................................................................... 475 A. Ramar and R. Schäublin
TEM investigation on the acicular ferrite precipitation in γ’-Fe4N nitride........... 477 X.-C. Xiong, A. Redjaïmia, and M. Gouné
Orientation Relationships between the δ-ferrite Matrix in a Duplex Stainless Steel and its Decomposition Products: the Austenite and the χ and R Frank-Kasper Phases ............................................. 479 A. Redjaïmia, T. Otarola, and A. Mateo
TEM study of localized deformation-induced disorder in intermetallic alloys of L12 structure........................................................................................................... 481 C. Rentenberger, C. Mangler, and H.P. Karnthaler
SEM and TEM study of dynamic recrystallisation of zirconium alloy.................. 483 L. Saintoyant, L. Legras, and Y. Brechet
Effects of solution treatment and test temperature on tensile properties of high strength high Mn austenitic steels ................................................................ 485 K. Phiu-on, W. Bleck, A. Schwedt, and J. Mayer
Microstructure evolution during Ni/Al multilayer reactions ................................. 487 S. Simões, F. Viana, A.S. Ramos, M.T. Vieira, and M.F. Vieira
TEM investigation of severely deformed NiTi and NiTiHf shape memory alloys .................................................................................................. 489 G. Steiner, M. Peterlechner, T. Waitz, and H.P. Karnthaler
TEM studies of nanostructured NiTiCo shape memory alloy for medical applications............................................................................................. 491 D. Stróż and Z. Lekston
TEM investigations of microalloyed steels with Nb, V and Ti after different treatments .......................................................................................... 493 G. Szalay, R. Grill, K. Spiradek-Hahn, and M. Brabetz
Initial Stages of the ω Phase Transformation .......................................................... 495 R. Tewari, K.V. Manikrishna, G.K. Dey, and S. Banerjee
TEM study of the Ni-Ti shape memory micro-wire ................................................ 497 H. Tian, D. Schryvers, and J. Van Humbeeck
Multi-scale observations of deformation twins in Ti6Al4V .................................... 499 W. Tirry, F. Coghe, L. Rabet, and D. Schryvers
Nd:YAG laser joining between stainless steel and nickel-titanium shape memory alloys .................................................................................................. 501 J. Vannod, A. Hessler-Wyser, and M. Rappaz
XX
Content
Focused Ion Beam application on the investigation of tungsten-based materials for fusion application.................................................. 503 L. Veleva, R. Schäublin, A. Ramar, Z. Oksiuta, and N. Baluc
HRTEM of NiTi shape memory alloys made amorphous by high pressure torsion............................................................................................. 505 T. Waitz, K. Tsuchiya, M. Peterlechner, and H.P. Karnthaler
Is the lattice structure of the martensite in nanocrystalline NiTi base centred orthorhombic? .............................................................................................. 507 T. Waitz
TEM study of the NiTi shape memory thin film...................................................... 509 B. Wang, A. Safi, T. Pardoen, A. Boe, J.P. Raskin, X. Wang, J.J. Vlassak, and D. Schryvers
Sub-nano analysis of fine complex carbide in high strength steel with probe Cs (S)TEM ............................................................................................... 511 K. Yamada, E. Hamada, K. Sato, and K. Inoke
Characterization of morphology and microstructure of different kinds of materials at NTNU Mater Sci EM Lab ................................................................ 513 Y.D. Yu, T. Nilsen, M.P. Raanes, J. Hjelen, and J.K. Solberg
Characterization of a Ti64Ni20Pd16 thin film by transmission electron microscopy........................................................................ 515 R. Zarnetta, E. Zelaya, G. Eggeler, and A. Ludwig
Analytical electron microscopy investigations of a microstructure of single and polycrystalline β-Mg2Al3 Samson phase............................................. 517 A. Zielińska-Lipiec, B. Dubie,l and A. Czyrska-Filemonowicz
M3.2 Ceramic materials Grain boundary interfaces in ceramics .................................................................... 519 D.J.H. Cockayne, S.-J. Shih, K. Dudeck, and N. Young
Structure and chemistry of nanometer-thick intergranular films at metal-ceramic interfaces........................................................................................ 521 W.D. Kaplan and M. Baram
Studying nanocrystallization behaviour of different inorganic glasses using Transmission Electron Microscopy ................................................................ 523 Somnath Bhattacharyya, Th. Höche, C. Bocker, C. Rüssel, A. Duran, N. Hémono, F. Muñoz, M.J. Pascual, K. Hahn, and P.A. van Aken
HRTEM and Diffraction Analysis of Surface Phases in Nanostructured LiMn1.5Ni0.5O4 Spinel.................................................................................................. 525 F. Cosandey, N. Marandian Hagh, and G.G. Amatucci
Content
XXI
The structural origin of the antiferroelectric properties and relaxor behavior of Na0.5Bi0.5TiO3 ..................................................................... 527 V. Dorcet, G. Trolliard, and P. Boullay
Electron beam probing of insulators ........................................................................ 529 H.-J. Fitting, N. Cornet, M. Touzin, D. Goeuriot, C. Guerret-Piécourt, D. Juvé, and D. Tréheux
Characterization of Ge-based clathrates oxidized in air by means of TEM and SEM...................................................................................................................... 531 C. Hébert, B. Bartova, M. Cantoni, U. Aydemir, and M. Baitinger
Microstructure analysis of thin Cr2AlC films deposited at low temperature by magnetron sputtering............................................................................................ 533 R. Iskandar, D.P. Sigumonrong, J.M. Schneider, and J. Mayer
Study of structural variation in YBaCo4O7+δ by electron diffraction .................... 535 Y. Jia, H. Jiang, M. Valkeapää, M. Karppinen, and E.I. Kauppinen
Exsolution phenomena in glass-ceramic systems..................................................... 537 I. Tsilika, Ph. Komninou, G.P. Dimitrakopulos, Th. Kehagias, and Th. Karakostas
Transmission Electron Microscopy Studies of Lead-Free Ferroelectrics in the System BNT-BT-KNN ..................................................................................... 539 H.-J. Kleebe, J. Kling, L. Schmitt, S. Lauterbach, and H. Fuess
ReO3-related aluminum tungsten oxides showing a novel type of crystallographic shear structure........................................................................... 541 F. Krumeich and G.R. Patzke
Structural Characterisation by TEM of a New Homologous Series Bi2n+4MonO6(n+1); n=3,4,5 and 6.................................................................................. 543 A.R. Landa-Canovas, J. Hernández-Velasco, E. Vila, J. Galy, and A. Castro
Structural characterisation of a new rich iron layered oxide TlεSr25-εFe30O76-ξ .... 545 C. Lepoittevin, S. Malo, S. Hebert, M. Hervieu, and G. Van Tendeloo
EBSD studies of stress concentrations in ferroelectrics .......................................... 547 I. MacLaren, M.U. Farooq, R. Villaurrutia, T.L. Burnett, T.P. Comyn, A.J. Bell, H. Kungl, and M.J. Hoffmann
High-resolution pictures of nucleation growth triangle of 180° ferroelectric domain wall in a thin film of LiTaO3 obtained by Lorentz DPC-STEM............... 549 T. Matsumoto, M. Koguchi, and Y. Takahashi
Size and structure of barium halide nano-crystals in optically active fluorozirconate-based glasses .................................................................................... 551 P.T. Miclea, B. Ahrens, C. Eisenschmidt, and S. Schweizer
Domain Structure And Microstructure Development of BaTiO3 Doped With Rare-Earth Dopants ......................................................................................... 553 V. Mitic, V.B. Pavlovic, V. Paunovic, M. Miljkovic, B. Jordovic, and Lj. Zivkovic
XXII
Content
SEM and EDS Analysis of BaTiO3 Doped With Yb2O3 and Ho2O3 ....................... 555 V. Mitic, V.B. Pavlovic, V. Paunovic, M. Miljkovic, B. Jordovic, and Lj. Zivkovic
Structure and superconductivity of Pr-Ba-Cu-O crystals prepared by ambient pressure synthesis using citrate pyrolysis method............................... 557 K. Nishio, T. Isshiki, T. Shima, and M. Hagiwara
Electron Diffuse Scattering in epitaxially grown SrTiO3 thin film ........................ 559 F. Pailloux and J. Pacaud
Investigation of the hydration of calciumsulfate hemihydrates with different microscopic methods.......................................................................... 561 C. Pritzel and R. Trettin
Investigation of holes in calciumsulfate-hemihydrate crystals by different microscopic methods ............................................................................. 563 C. Pritzel and R. Trettin
Analytical and high-resolution TEM investigation of Boron-doped CeO2 ............ 565 B. Rahmati, G. Gregori, W. Sigle, C.T. Koch, P.A. van Aken, and J. Maier
Accommodation of the compositional variations in the Ca1-xSrxMnO3-δ (0≤x≤1, 0≤δ≤0.5) system............................................................................................. 567 S. de Dios, J. Ramírez-Castellanos, A. Varela, M. Parras, and J.M. González Calbet
Evidence of SrO(SrTiO3)n Ruddlesden-Popper Phases by High Resolution Electron Microscopy and Holography .................................... 569 M. Reibold, E. Gutmann, A.A. Levin, A. Rother, D.C. Meyer, and H. Lichte
New Barium Antimony Aluminates evidenced by TEM techniques...................... 571 R. Retoux, A. Letrouit, M. Hervieu, and S. Boudin
(Multi-)ferroic domain walls– a combined ab-initio and microscopical investigation ................................................................................ 573 A. Rother, S. Gemming, D. Geiger, and N. Spaldin
Diagnostic of Li battery cathode by EELS, first principles calculation and spectrum-imaging with multi-variate analysis ................................................. 575 K. Tatsumi, Y. Sasano, S. Muto, T. Sasaki, Y. Takeuchi, K. Horibuchi, and Y. Ukyo
Local electronic structure analysis on Ce3+-containing materials by TEM-EELS and first principles calculations...................................................... 577 K. Tatsumi, I. Nishida, and S. Muto
Local chemical inhomogeneities in NaNb1-xTaxO3 as observed by HRTEM and HAADF-STEM.................................................................................................... 579 A. Torres-Pardo, E. García-González, J.M. González-Calbet, F. Krumeich, and R. Nesper
The influence of lanthanum doping on the structure of PbZr0.9Ti0.1O3 ceramics.......................................................................................... 581 R. Villaurrutia, I. MacLaren, and A. Peláiz-Barranco
Content
XXIII
Anomalous absorption of electrons during electron diffraction on BaTiO3 single crystals near phase transition at 120°C ...................................... 583 A. Wall
Template-assisted synthesis and characterization of SrTiO3 nanostructures........................................................................................... 585 K. Žagar, S. Šturm, and M. Čeh
(S)TEM/EELS characterisation of a multilayer C/Cr PVD coating ...................... 587 Z. Zhou, W.M. Rainforth, M. Gass, A. Bleloch, and P.Eh. Hovsepian
M3.3 Magnetic materials High resolution imaging of magnetic structures in a TEM – what is possible? .... 589 J. Zweck
Phase segregation leading to spontaneous outcropping of (Sr,La)Ox dots in La1-xSrxMnO3 films ................................................................................................ 591 P. Abellan, F. Sandiumenge, C. Moreno, M.J. Casanove, T. Puig, and X. Obradors
Microstructure of epitaxially strained LaCoO3 thin films...................................... 593 L. Dieterle, D. Gerthsen, and D. Fuchs
Are the samples really flat? Influence of the supporting membrane on the magnetization of patterned micromagnets ................................................... 595 C. Dietrich and J. Zweck
HRTEM characterization of core-shell Fe@C and Fe@SiO2 magnetic nanoparticles prepared by the arc-discharge plasma method................................ 597 Rodrigo Fernández-Pacheco, Manuel Arruebo, Jordi Arbiol, Clara Marquina, Jesús Santamaría, and M. Ricardo Ibarra
Nanofabrication of ferromagnetic nanotips and nanobridges by 2D and 3D electron-beam cutting ................................................................................... 599 T. Gnanavel, Z. Saghi, Y. Peng, B.J. Inkson, M.R.J. Gibbs, and G. Möbus
An investigation into the crystallization of the MgO barrier layer of a magnetic tunnel junction .................................................................................... 601 V. Harnchana, A.P. Brown, R.M. Brydson, A.T. Hindmarch, and C.H. Marrows
FeCoAlN films with induced magnetic anisotropy .................................................. 603 A. Lančok, M. Klementová, M. Miglierini, F. Fendrych, K. Postava, J. Kohout, and O. Životský
The martensitic microstructure of 5M and NM martensites in off-stoichiometric Ni2MnGa ferromagnetic shape memory alloys..................... 605 Pallavi Sontakke, Amita Gupta, and Madangopal Krishnan
TEM characterization of nanometer-sized Fe/MgO granular multilayer thin films grown by pulsed laser deposition............................................................. 607 C. Magén, E. Snoeck, A. García-García, J.A. Pardo, P.A. Algarabel, P. Štrichovanec, A. Vovk, L. Morellón, J.M. De Teresa, and M.R. Ibarra
XXIV
Content
Structural modification and self-assembly of nanoscale magnetite synthesised in the presence of an anionic surfactant ................................................................... 609 S. Malik, I.J. Hewitt, and A.K. Powell
Electron microscopy phase retrieval of perpendicular magnetic anisotropy (PMA) FePd alloys ..................................................................................................... 611 A. Masseboeuf, C. Gatel, A. Marty, E. Snoek, and P. Bayle-Guillemaud
Magnetic domain wall propagation in nanostructures of alloys with perpendicular magnetic anisotropy.................................................................. 613 A. Masseboeuf, A. Mihaï, J.P. Attané, J.C. Pillet, P. Warin, A.L. Vila, G. Gaudin, M. Miron, B. Rodmacq, E. Gautier, A. Marty, and P. Bayle-Guillemaud
The effect of annealing in the microstructure and magnetic properties of NiCuZn ferrites ...................................................................................................... 615 D. Sakellari, V. Tsakaloudi, V. Zaspalis, and E.K. Polychroniadis
Microstructural and compositional analyses of nano-structured Co-Pt thin films ..................................................................................................................... 617 Z. Samardžija, K. Žužek Rožman, and S. Kobe
L10-type ordered structure of FePd nanoparticles studied by high-resolution transmission electron microscopy ............................................. 619 K. Sato, T.J. Konno, and Y. Hirotsu
Structural and chemical characterization of Co-doped ZnO layers grown on Si and sapphire ...................................................................................................... 621 R. Schneider, L.D. Yao, D. Gerthsen, G. Mayer, M. Fonin, and U. Rüdiger
TEM studies of cobalt-doped zinc oxide films ......................................................... 623 J. Simon, K. Nielsen, M. Opel, S.T.B. Goennenwein, R. Gross, and W. Mader
Nanocrystallization of amorphous Fe40Ni38B18Mo4 alloy ........................................ 625 D. Srivastava, A.P. Srivastava, and G.K. Dey
Structural and compositional properties of Sm-Fe-Ta magnetic nanospheres prepared by pulsed-laser deposition at 157 nm in a N2 atmosphere...................... 627 S. Šturm, K. Žužek Rožman, E. Sarantopoulou, and S. Kobe
Characterization of Ni-Mn-Ga magnetic shape memory alloys using electron holography and Lorentz microscopy ............................................... 629 K. Vogel, M. Linck, Ch. Matzeck, A. Rother, D. Wolf, and H. Lichte
Energy Loss Magnetic Chiral Dichroïsm (EMCD) for magnetic material............ 631 B. Warot-Fonrose, L. Calmels, C. Gatel, F. Houdellier, V. Serin, and E. Snoeck
M3.4 Dislocations, interfaces and other defects Determining the nanoscale chemistry and behavior of interfaces and phases in Al-Si(-Cu-Mg) nanoparticles using in-situ TEM................................................. 633 J.M. Howe, S.K. Eswaramoorthy, and G. Muralidharan
Content
XXV
Dislocations in AlPdMn quasicrystals: contrast in TEM and physical properties .............................................................................................. 635 D. Caillard and F. Mompiou
Characterization of a-plane GaN films grown on r-plane sapphire substrate by electron microscopy .............................................................................................. 637 Y. Arroyo Rojas Dasilva, T. Zhu, D. Martin, N. Grandjean, and P. Stadelmann
A method for atomistic/continuum analysis of defects in large HRTEM images ............................................................................................ 639 A. Belkadi, G.P. Dimitrakopulos, J. Kioseoglou, G. Jurczak, T.D. Young, P. Dluzewski, and Ph. Komninou
High resolution electron microscopy of interfaces in ultrafine microstructures of Zr and Ti based alloys ........................................... 641 G.K. Dey, S. Neogy, R.T. Savalia, R. Tewari, D. Srivastava, and S. Banerjee
Anisotropic strain relaxation in (110) La2/3Ca1/3MnO3 thin films .......................... 643 S. Estrade, I.C. Infante, F. Sanchez, J. Fontcuberta, J. Arbiol, and F. Peiró
Metadislocations in complex metallic alloys: core structures investigated by aberration-corrected scanning transmission electron microscopy ................... 645 M. Feuerbacher, L. Houben, and M. Heggen
TEM of high pressure torsion processed intermetallic Zr3Al................................. 647 D. Geist, C. Rentenberger, and H.P. Karnthaler
Multiscale characterisation of the plasticity of Fe-Mn-C TWIP steels .................. 649 H. Idrissi, L. Ryelandt, K. Renard, S. Ryelandt, F. Delannay, D. Schryvers, and P.J. Jacques
Misfit analysis of the InN/GaN interface through HRTEM image simulations ....................................................................................................... 651 J. Kioseoglou, G.P. Dimitrakopulos, Th. Kehagias, E. Kalessaki, Ph. Komninou, and Th. Karakostas
Application of TEM for Real Structure Determination of Rare Earth Metal Compounds.............................................................................. 653 L. Kienle, V. Duppel, Hj. Mattausch, M.C. Schaloske, and A. Simon
Quantitative Dislocation Analysis of 2H AlN:Si grown on (0001) Sapphire ......... 655 O. Klein, J. Biskupek, U. Kaiser, S.B. Thapa, and F. Scholz
Transrotational crystals in crystallizing amorphous films: new solid state order or novel extended imperfection............................................. 657 V.Yu. Kolosov
Determination of precise orientation relationships between surface precipitates and matrix in a duplex stainless steel................................................... 659 Y. Meng, G. Nolze, W.Z. Zhang, L. Gu, and P.A. van Aken
Interfaces in Cu(In,Ga)Se2 thin film solar cells ....................................................... 661 G. Östberg and E. Olsson
XXVI
Content
In-situ electron beam irradiation of nanopipes in GaN .......................................... 663 F. Pailloux and J.-F. Barbot
The atomic structure of an incommensurate (001)-(110) Si grain boundary resolved thanks to a probe Cs-corrector .................................................................. 665 J.L. Rouviere, F. Lançon, K. Rousseau, D. Caliste, and F. Fournel
Atomic structure and dopant segregation of [0001] tilt grain boundaries in ZnO bicrystals ........................................................................................................ 667 Y. Sato, T. Mizoguchi, J.P. Buban, N. Shibata, T. Yamamoto, T. Hirayama, and Y. Ikuhara
TEM study of strain and defect engineering with diluted nitride semiconductors ......................................................................... 669 J. Schöne, E. Spiecker, F. Dimroth, A.W. Bett, and W. Jäger
Investigation of the Co-Precipitation of Copper and Nickel in Silicon by Means of Transmission Electron Microscopy..................................................... 671 C. Rudolf, L. Stolze, and M. Seibt
Micro-structure analysis of a friction-stir welded 2024 aluminium alloy using electron microscopy.......................................................................................... 673 E. Sukedai, T. Maebara, and T. Yokayama
Deformation defects in a metastable β titanium alloy............................................. 675 H. Xing and J. Sun
Defect generation and characterization in 4H-SiC.................................................. 677 J.P. Ayoub, M. Texier, G. Regula, M. Lancin, and B. Pichaud
Investigation of defects in polymorph B enriched zeolite Beta............................... 679 D. Zhang, J. Sun, S. Hovmöller, and X. Zou
M3.5 Coatings and graded materials Optimizing electron diffraction and EDS for phase identification in complex structures: application to multilayered Ti-Ni-P coatings .................... 681 P.A. Buffat and A. Czyrska-Filemonowicz
Advanced analytical transmission electron microscopy to investigate the nano-graded materials properties ...................................................................... 683 M. Cheynet, S. Pokrant, L. Joly-Pottuz, and J.M. Martin
Characterisation of Nickel Nanocomposites by SEM, TEM and EBSD................ 685 D. Dietrich, Th. Lampke, B. Wielage, D. Thiemig, and A. Bund
Characterisation of Gold Nanocomposites by SEM, TEM and EBSD .................. 687 D. Dietrich, Th. Lampke, B. Wielage, P. Cojocaru, and P.L. Cavallotti
Alumina Coatings as Protection against Corrosive Atmosphere ........................... 689 I. Dörfel, R. Sojref, M. Dressler, D. Hünert, and M. Nofz
Content
XXVII
Advanced Multilayer Systems for X-ray Optics: Quality Assessment by TEM ....................................................................................................................... 691 D. Häussler, W. Jäger, E. Spiecker, B. Ögüt, U. Ross, J. Wiesmann, and M. Störmer
Surface investigation of SU-8 by atomic force and scanning electron microscopy ............................................................................ 693 Th. Kups, Chr. Kremin, M. Hoffmann, and L. Spieß
SEM and TEM investigations of electrophoretical deposited Si3N4 and SiC particles in siloxane of steel substrate ........................................................ 695 Th. Kups, A. Knote, and L. Spieß
Contribution of electron microscopy techniques to the chemical and structural characterization of TiC/a-C nanocomposite coatings .................... 697 C. López-Cartes, D. Martínez-Martínez, J.C. Sánchez-López, and A. Fernández
TEM investigations of the Ti/TiN multilayered coatings deposited on the Ti-6Al-7Nb alloy.............................................................................................. 699 T. Moskalewicz, H.J. Penkalla, and A. Czyrska-Filemonowicz
Microstructural examination of Al and Cr alloyed zinc coatings on low carbon steels.................................................................................................... 701 D. Chaliampalias, G. Vourlias, E. Pavlidou, K. Chrissafis, G. Stergioudis, and S. Skolianos
Study of the structure and high temperature oxidation resistance of high alloyed tool steels ........................................................................................... 703 E. Pavlidou, D. Chaliampalias, G. Vourlias, and K. Chrissafis
A comparative study of NiCrBSi and Al coated steels with thermal spray process in different environments............................................................................. 705 D. Chaliampalias, G. Vourlias, E. Pavlidou, K. Chrissafis, G. Stergioudis, and S. Skolianos
Microscopical study of the influence of zinc addition on the structure of WO3.... 707 K. Nikolaidis, D. Chaliampalias, G. Vourlias, E. Pavlidou, and G. Stergioudis
Microstructural Studies by Electron Microscopy Techniques of TiAlSiN Nanostructured Coatings........................................................................................... 709 V. Godinho, T.C. Rojas, M.C. Jimenez, M.P. Delplancke-Ogletree, and A. Fernández
Structural and interface studies of a nano-scale TiAlYN/CrN/alumina coating ................................................................................... 711 I.M. Ross, W.M. Rainforth, C. Strondl, F. Papa, and R. Tietema
An investigation of SiC-fiber coatings ...................................................................... 713 T. Toplišek, Z. Samardžija, G. Dražić, S. Kobe, and S. Novak
HRTEM-EELS study of atomic layer deposited thin rare earth oxide films for advanced microelectronic devices ....................................................................... 715 S. Schamm, P.E. Coulon, and L. Calmels
XXVIII
Content
New Fullerene like materials for tribological applications: TEM and EELS study................................................................................................ 717 Virginie Serin, Nathalie Brun, and Ch. Colliex
Phase determination of nanocrystalline Al-Cr-O coatings by analytical TEM...................................................................................................... 719 J. Thomas, J. Ramm, B. Arnold, B. Widrig, and T. Gemming
M3.6 Biomaterials Bioinspired synthesis of nanostructures based on S-layer lattices ......................... 721 D. Pum, N. Ilk, and U.B. Sleytr
Direct Imaging of Carbon Nanoparticles inside Human Cells ............................... 723 A.E. Porter, C. Cheng, M. Gass, K. Muller, J. Skepper, P. Midgley, and M. Welland
Micro- and Nano-Textured Surfaces on Ti-Implants Made by Various Methods ................................................................................................... 725 U. Beck, R. Lange, and H.-G. Neumann
Determination of the biocompatibility of biomaterials by scanning electron microscopy (SEM) .................................................................. 727 M. Bovi, N. Gassler, and B. Hermanns-Sachweh
Quantitative evaluation of the long-term marginal behaviour of filling restorations of human teeth using three-dimensional scanning electron microscopy.................................................................................................... 729 W. Dietz, S. Nietzsche, R. Montag, P. Gaengler, and I. Hoyer
The analysis of Si doped hydroxyapatite coatings using FIBSEM, TEM and RHEED ................................................................................................................ 731 H.K. Edwards, S. Coe, T. Tao, M.W. Fay, C.A. Scotchford, D.M. Grant, and P.D. Brown
Electron microscopic investigations of the polymer/mineral composite material nacre............................................................................................................. 733 K. Gries, R. Kröger, C. Kübel, M. Fritz, and A. Rosenauer
Studies on the microstructure of fresh-cut melon ................................................... 735 I. Hernando, L. Alandes, A. Quiles, and I. Pérez-Munuera
Ceramic-loaded mineralizing bioresorbable polymers for orthopaedic applications...................................................................................... 737 L.W. Hobbs, T. Lim, A. Porter, H. Wang, M. Walton, and N.J. Cotton
AFM and TEM study of Ag coated insulin-derived amyloid fibrils ...................... 739 M. Gysemans, J. Snauwaert, C. Van Haesendonck, F. Leroux, B. Goris, S. Bals, and G. Van Tendeloo
Transmission Electron Microscopy studies of bio-implant interfaces using Focused Ion Beam microscopy for sample preparation................................ 741 F. Lindberg, A. Palmquist, L. Emanuelsson, J. Heinrichs, R. Brånemark, F. Ericson, P. Thomsen, and H. Engqvist
Content
XXIX
AFM and SEM of Wax Crystallisation on Artificial Surfaces Controlled by Temperature and Solvents ................................................................................... 743 A. Niemietz, W. Barthlott, K. Wandelt, and K. Koch
Characterization of layer-by-layer microcapsules made of hyaluronic acid by CLSM, SEM and TEM ......................................................................................... 745 I. Pignot-Paintrand, A. Szarpak, and R. Auzely-Velty
Atomic force microscopy analysis of crystalline silicon functionalization with oligonucleotides .................................................................................................. 747 A. Ponzoni, G. Faglia, M. Ferroni, G. Sberveglieri, A. Flamini, G. Andreano, and L. Cellai
Hidden hierarchy of microfibrils within fluorapatite gelatine nanocomposites induced by intrinsic electric dipole fields ..................................... 749 P. Simon and R. Kniep
M4
Soft Matter and Polymers
Self-assembled block copolymer structures studied by transmission electron microtomography ........................................................................................ 751 H. Jinnai, T. Kaneko, C. Abetz, and V. Abetz
Quantitative chemistry and orientation of polymers in 2-d and 3-d by scanning transmission X-ray microscopy............................................................ 753 A.P. Hitchcock, G.A. Johansson, D. Hernández Cruz, E. Najafi, J. Li and and H. Stöver
Characterization of cavitation processes in filled semi-crystalline polymers........ 755 F. Addiego, J. Di Martino, D. Ruch, A. Dahoun, and O. Godard
Quantitative analysis of protein gel structure by confocal laser scanning microscopy .................................................................................................. 757 K. Ako, L. Bécu, T. Nicolai, J.-C. Gimel, and D. Durand
Thermal stability of organic solar cells: the decay in photocurrent linked with changes in active layer morphology ................................................................. 759 S. Bertho, I. Haeldermans, A. Swinnen, J. D’Haen, L. Lutsen, T.J. Cleij, J. Manca, and D. Vanderzande
Determining absorptive potential variation in electron beam sensitive specimens using a single energy-filtered bright-field TEM image ......................... 761 S. Bhattacharyya and J.R. Jinschek
Elemental distribution of soft materials with newly designed 120kV TEM/STEM .................................................................................... 763 C. Hamamoto, N. Endo, H. Nishioka, T. Ishikawa, Y. Ohkura, and T. Oikawa
Preparation of titanate nanotubes and their polymer composites ......................... 765 D. Kralova, N. Neykova, and M. Slouf
XXX
Content
Nanometer size wear debris generated from ultrahigh molecular weight polyethylene in vivo .................................................................................................... 767 M. Lapcikova, M. Slouf, J. Dybal, E. Zolotarevova, G. Entlicher, D. Pokorny, J. Gallo, and A. Sosna
Analysis of nano-composites based on carbon nanoparticles imbedded in polymers.................................................................................................................. 769 Kangbo Lu, Joachim Loos, Sourty Erwan, and Dong Tang
New developments in SEM for in situ tensile tests on polymers............................. 771 P. Jornsanoh, G. Thollet, C. Gauthier, and K. Masenelli-Varlot
A study of the spatial distributions of the carbon blacks in polypropylene composites using TEM-Tomography and quantitative image analysis ................. 773 H. Matsumoto, H. Sugimori, T. Tanabe, Y. Fujita, H. Sano, and H. Jinnai
A study of the chain-folded lamellae structure and its array in the isotactic polypropylene spherulites by HAADF-STEM and HV-TEM Tomography techniques.................................................................... 775 H. Matsumoto, M. Song, H. Sano, M. Shimojo, and K. Furuya
Microstructural analysis of ultra-thin nanocomposite layers fabricated by Cu+ ion implantation in inert polymers............................................................... 777 G. Di Girolamo, E. Piscopiello, M. Massaro, E. Pesce, C. Esposito, L. Tapfer, and M. Vittori Antisari
In-situ experiments on soft materials in the environmental SEM – Reliable results or merely damage?......................................................................................... 779 P. Poelt, H. Reingruber, A. Zankel, and C. Elis
Structural studies on V-amylose inclusion complexes............................................. 781 J.L. Putaux, M. Cardoso, M. Morin, D. Dupeyre, and K. Mazeau
Multilamellar nanoparticles from PS-b-PVME copolymers .................................. 783 C. Lefebvre, J.-L. Putaux, M. Schappacher, A. Deffieux, and R. Borsali
TEM/SEM characterisation of hybrid titanoniobiates used as fillers for thermoplastic nanocomposites ............................................................................ 785 R. Retoux, S. Chausson, L. Le Pluart, J.M. Rueff, and P.A. Jaffres
Phase transitions and ordering in liquid crystals – a case study ............................ 787 A.K. Schaper
Study of degradation and regeneration of silicon polymers using cathodoluminescence........................................................................................ 789 P. Schauer, P. Horak, F. Schauer, I. Kuritka, and S. Nespurek
Orthogonal self-assembly of surfactants and hydrogelators: towards new nanostructures...................................................................................... 791 M.C.A. Stuart, A.M.A. Brizard, E.J. Boekema, and J.H. van Esch
Content
XXXI
Structure of particles formed during Se redox process in aqueous polymer solutions .................................................................................... 793 E.I. Suvorova, V.V. Klechkovskaya, M. Cantoni, and P.A. Buffat
Exploring the 3D organisation of high-performance organic solar cells ............... 795 S. van Bavel, E. Sourty, B. de With, and J. Loos
Morphological study on three kinds of two-dimensional spherulites of PBT ....... 797 T. Yoshioka and M. Tsuji
Solution-Grown Crystals of Optically Active Propene–Carbon Monoxide Copolymer................................................................................................................... 799 T. Yoshioka, N. Kosaka, A. Nakayama, A.K. Schaper, W. Massa, T. Hiyama, K. Nozaki, and M. Tsuji
M5
Materials in Mineralogy, Geology and Archaeology
New insights into ultra-high pressure metamorphism from TEM studies ............ 801 F. Langenhorst and A. Escudero
Characterization of a (021) twin in coesite using LACBED and precession electron diffraction........................................................................... 803 P. Cordier, D. Jacob, and H.-P. Schertl
Rubens in the Prado National Museum: analytical characterization of ground layers.......................................................................................................... 805 M.I. Báez, L. Vidal, M.D. Gayo, J. Ramírez-Castellanos, J.L. Baldonedo, and A. Rodríguez
Development of the FIB-cryo-SEM approach for the in-situ investigations of the elusive nanostructures in wet geomaterials ................................................... 807 G. Desbois and J.L. Urai
TEM applied on the interface characterisation of the replacement reaction chlorapatite by hydroxyapatite ................................................................................. 809 U. Golla-Schindler, A. Engvik, H. Austrheim, and A. Putnis
Quantitative study of valence states of zirconolites ................................................. 811 U. Golla-Schindler and P. Pöml
Study of Organic Mineralogical Matter by Scanning Probe Microscopy ............. 813 Ye.A. Golubev and O.V. Kovaleva
Research of Nanoparticle Aggregates from Water Colloidal Solutions of Natural Carbon Substances and Fullerenes by Atomic Force Microscopy ...... 815 Ye.A. Golubev and N.N. Rozhkova
Diffusion in Synthetic Grain Boundaries ................................................................. 817 K. Hartmann, R. Wirth, R. Dohmen, G. Dresen, and W. Heinrich
XXXII
Content
An examination of Van Gogh’s painting grounds using analytical electron microscopy – SEM/FIB/TEM/EDX .......................................................................... 819 R. Haswell, U. Zeile, and K. Mensch
Amorphisation in fresnoite compounds – a combined ELNES and XANES study....................................................................................................... 821 Th. Höche, F. Heyroth, P.A. van Aken, F. Schrempel, G.S. Henderson, and R.I.R. Blyth
TEM study of Comet Wild 2 pyroxene particles collected during the stardust mission ....................................................................................... 823 D. Jacob, J. Stodolna, and H. Leroux
The mechanism of ilmenite leaching during experimental alteration in HCl-solution ........................................................................................................... 825 A. Janßen, U. Golla-Schindler, and A. Putnis
Microstructure and Texture from Experimentally Deformed Hematite Ore ....... 827 K. Kunze, H. Siemes, E. Rybacki, E. Jansen, and H.-G. Brokmeier
Identifying pigments in the temple of Seti I in Abydos (Egypt) ............................. 829 E. Pavlidou, H. Marey Mahmoud, E. Roumeli, F. Zorba, K.M. Paraskevopoulos, and M.F. Ali
Nanostructural study of ground layers of canvas of Rubens at “El Prado” National Museum ............................................................................... 831 J. Ramírez-Castellanos, J.L. Baldonedo, M.I. Báez, L. Vidal, M.D. Gayo, and M.J. García
Micro- and nano-diamond particles in carbon spherules found in soil samples ............................................................................................................. 833 Z. Yang, D. Schryvers, W. Rösler, N. Tarcea, and J. Popp
The use of FIB/TEM for the study of radiation damage in radioactive/non-radioactive mineral assemblages............................................... 835 A.-M. Seydoux-Guillaume, J.-M. Montel, and R. Wirth
Non-destructive 3D measurements of sandstone’s internal micro-architecture using high resolution micro-CT ................................................................................ 837 E. Van de Casteele, S. Bugani, M. Camaiti, L. Morselli, and K. Janssens
Author Index............................................................................................................... 839 Subject Index .............................................................................................................. 859
1
Direct observation of atomic defects in carbon nanotubes and fullerenes K. Suenaga National Institute of Advanced Industrial Science and Technology (AIST) and the Japan Science and Technology Agency (JST), Tsukuba, 305-8565, Japan
[email protected] Keywords: defect, nanotube, fullerene
The diversified properties of carbon nano-structures (nanotubes, fullerenes and their derivatives) are related to their polymorphic arrangement of carbon atoms. Therefore the direct observation of carbon network, such as defects or chirality, is of great consequence in both scientific and technological viewpoints in order to predict the physical and chemical properties. In order to identify the local configuration of pentagons and hexagons in carbon nanostructures, an electron microscope with higher spatial resolution and higher sensitivity is definitively required. Since the spatial resolution of the conventional TEM is limited by the spherical aberration coefficient (Cs) of its objective lens and the wave length (λ) of incident electron beam, the Cs must be minimized to achieve the best performance because the reduction of the λ is detrimental to the high sensitivity to visualize individual carbon atoms. A highresolution transmission electron microscope (HRTEM, JEOL-2010F) equipped with a Cs corrector (CEOS) was operated at a moderate accelerating voltage (120kV). The Cs was set to 0.5 ~ 10 µm in this work. The HRTEM images were digitally recorded under a slightly under-focus condition (Δf = -2 to -7 nm) where the point resolution of 0.14 nm was achieved at 120kV. The spatial resolution of 0.14 nm (a typical C-C bond length) obtained at a moderate accelerating voltage provides us a great advantage because we can realize the visualization of carbon atomic arrangement without massive electron irradiation damage. Here we show some examples for atomic-level characterization of carbon nanostructures. The C60 and C80 fullerene molecule has been successfully identified its structure and orientation at a single-molecular basis (1, 2). Also the active topological defects have been eventually caught red-handed (3, 4). The technique can be widely applicable to visualize a biological activity, at an atomic level, for which any conformation change of the C-C bonds is responsible. The cis-/trans-isomerization of retinal molecules have been successfully visualized (5). 1. 2. 3. 4. 5.
Z. Liu, K. Suenaga and S. Iijima, J. Am. Chem. Soc., 129 (2007) 6666. Y. Sato, K. Suenaga, S. Okubo, T. Okazaki and S. Iijima, Nano Letters, 7 (2007) 3704. K. Suenaga, H. Wakabayashi, M. Koshino, Y. Sato, K. Urita and S. Iijima, Nature Nanotech. 2 (2007) 358. C.-H. Jin, K. Suenaga and S. Iijima, Nature Nanotech. 3 (2008) 17. Z. Liu, K. Yanagi, K. Suenaga, H. Kataura and S. Iijima, Nature Nanotech. 2 (2007) 422.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 1–2, DOI: 10.1007/978-3-540-85226-1_1, © Springer-Verlag Berlin Heidelberg 2008
2
6.
The supports of the JST-CREST, JST-ERATO, KAKENHI and JSPS are kindly acknowledged.
Figure 1. a, A 5–7 pair defect found in an SWNT after heat treatment at 2,273 K. b, An enlarged image of the area enclosed by the green line in a) in which the 5–7–7–5 defect can be more clearly seen. c, The black dots indicate the hexagons with six neighbors, the two red dots have seven neighbors, and the two black dots with circles have five neighbors.
Figure 2. a, The Stone-Wales (SW) transformation leading to the 5–7–7–5 defect, generated by rotating a C–C bond in a hexagonal network. b, HR-TEM image obtained for the atomic arrangement of the SW model. c, Simulated HR-TEM image for the model shown in b. (ref. 3)
3
Atomic studies on ferroelectric oxides by aberration corrected transmission electron microscopy K. Urban and C.L. Jia Institute for Solid State Research, Research Centre Jülich, and Ernst Ruska Centre for Microscopy and Spectroscopy with Electrons, D-52428 Jülich, Germany
[email protected] Keywords: Oxides, Interfaces, Defects
The advent of aberration-corrected transmission electron microscopy in 1998 [1] has provided materials science with entirely new tools for quantitative investigations. Four key innovations have to be mentioned: (1) The possibility to operate the electron microscope as a variable-sphericalaberration instrument allows to derive a new phase contrast theory optimizing both resolution and point spread [2]. In classical Scherzer phase contrast theory the radius of the point spread disc amounts to three times the Scherzer resolution limit. Besides the fact that information is lost by placing an aperture in the diffraction plane to keep the contrast oscillations in the contrast transfer function from affecting the images this point spread is a second disadvantage of the classical Scherzer approach to phase contrast. Both limitations can be substantially reduced in a new theory in which by both the objective lens defocus Z as well as CS the spherical aberration parameter adopt specific values. As a result the resolution limit coincides with the information limit and the point spread gets reduced to about one half of the latter making it an uncritical parameter in practice. (2) The negative spherical aberration imaging (NCSI) technique leads to enhanced contrast of atoms with low nuclear charge number [3]. It relies on two advantages compared to the classical Zernike technique. The shift of the phase of the diffracted waves is, in contrast to the classical Scherzer technique, in clockwise direction leading to white atom contrast. Furthermore the contrast is enhanced by a dynamic non-linear effect. Oxygen, nitrogen and even boron can be imaged directly even when these atomic species occur in close distance to heavy cations. (3) Essentially point-spread-free atomic images allow to measure occupancies of atomic columns, i.e. local concentrations, with lateral atomic resolution evaluating atomically resolved intensity measurements [4]. This means that high-resolution is not only a structural technique. From now on also local composition maps can be derived which are forming an excellent starting point for ab-initio calculations of interface-, boundary- and defect structures. (4) Measurements of atomic distances can be carried out at an accuracy of a few picometers [5]. This promises to measure structure-dependent physical properties directly on the atomic scale [6]. The technique of choice in ultra-high resolution transmission electron microscopy is to take a focal series of images on the basis of the NCSI technique which is forming the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 3–4, DOI: 10.1007/978-3-540-85226-1_2, © Springer-Verlag Berlin Heidelberg 2008
4
basis of a reconstruction of the electron exit-plane wave function (EPW) [7]. However, in order to arrive at the EPW all major aberrations up to fifth order have to be known or must be compensated. This has to be done by proper diagnostics and adjustment software. The focal series reconstruction allows for additional small corrections of the aberrations but it is by principle not suited to replace aberration correction in general. It should be noted that ultra-high resolution requires modelling of the structure and composition on the computer. The reconstructed EPW is in general not(!) sufficient to carry out high precision measurements since neither the specimen illumination conditions nor the thickness is known a priori. Both seriously affect the EPW. While the latter may permit qualitative interpretation, provided that the projected potential approximation is valid, it is required to do the complete computer fit up to the eventual real structure in order to be able to carry out the picometer-accuracy measurements in the computer. A first example in which the enhanced accuracy of aberration correction has been successfully applied is the investigation of the core structure of Σ3{111} twin boundaries in BaTiO3 [4]. It could be shown that the occupancy of the oxygen sites in the boundary is only 68 %, i.e. 32 % of the sites are left vacant. The corresponding change in the Ti-Ti separation across the boundary of +35 pm and of the Ba-Ba-separation of 17 pm is well described by ab-initio calculations [8]. In a recent study of PbZr0 2Ti0 8O3 (PZT) a new inversion domain boundary was discovered [6]. This longitudinal boundary is charged and presumably formed by the dynamics of domain growth during cooling from above the critical temperature. The boundary could be characterised on the atomic level and the polarisation shifts were measured atom by atom at an accuracy of a few picometers. From these data the polarisation could be calculated as a function of distance from the core of the domain. This is a first example that ferroelectric properties can be measured by ultra-high resolution atomic transmission electron microscopy. 1. 2. 3. 4. 5. 6. 7. 8.
M. Haider, S. Uhlemann, E. Schwan, H. Rose, B. Kabius, and K. Urban, Nature 392 (1998) p. 768. M. Lentzen, Ultramicroscopy 99 (2004) p. 211. C.L. Jia, M. Lentzen and K. Urban, Science 299 (2003) p. 870. C.L. Jia and K. Urban, Science 303 (2004) p. 2001. L. Houben, A. Thust and K. Urban, Ultramicroscopy 106 (2006), p. 200. C.L. Jia, S.B. Mi, K. Urban, I. Vrejoiu, M. Alexe and D. Hesse, Nature mat. 7 (2008) p. 57 K. Tillmann, A. Thust, and K. Urban, Microsc. Microanal. 10 (2004) p. 185. W.T. Geng, Y.J.Zhang & A.J. Freemann, Phys. Rev. B 63 (2000) p. 060101 R
5
Dark-field electron holography for the measurement of strain in nanostructures and devices M.J. Hÿtch, F. Houdellier, F. Hüe and E. Snoeck CEMES-CNRS, 29 rue Jeanne Marvig, 31055 Toulouse, France
[email protected] Keywords: strain, high-resolution, holography, semiconductors
We present a new method for measuring strain in nanostructures and electronic devices [1]. It is based on a combination of the moiré technique and off-axis electron holography. A hologram is created from the interference between the diffracted beam emanating from an unstrained region of crystal, which serves as the reference, and a beam from the region of interest containing strained crystal. A typical example for these two regions would be the substrate and an active region of a device. The aim is to measure geometric phase differences, from which the deformation can be calculated [2]. Naturally, any other phase contributions should be minimised, notably, dynamic phases due to thickness variations. For this reason, specimens should be prepared with suitably uniform thickness and regions exhibiting bend contours avoided. The technique has a number of advantages over geometric phase analysis (GPA) of high-resolution images for the study of transistors [3]. The specimens do not need to be so thin, being more like those of conventional TEM. Specimens are therefore easier to prepare and the effects of thin-film relaxation reduced. The major advantage, however, is the ability to analyse large regions of crystal at relatively low resolution. Results will be presented for different strained-silicon devices. TEM specimens are prepared by focussed ion beam (FIB) to thicknesses of about 200 nm. Observations are carried out on the SACTEM-Toulouse, a Tecnai (FEI) 200kV TEM equipped with a Cs corrector (CEOS), rotatable biprism and 2k CCD camera (Gatan). Strain fields are extracted using a modified version of GPA Phase 2.0 (HREM Research Inc.), a plug-in for DigitalMicrograph (Gatan). Typical fringe spacings are 1-2 nm and hologram widths from 300-400 nm allowing lengthwise fields of view of several microns. Figure 1 shows an example of a p-MOSFET with recessed Si80Ge20 source and drain [3]. Holograms were formed using the {111}, (004) and (220) diffracted beams (Figure 2a). The corresponding deformation map for the component parallel to the [220] direction, εxx, (Figure 2b) compares favourably with the result from finite element modelling (Figure 2c). In this case, the measurement precision is 0.2% for a spatial resolution of 4 nm. 1. 2. 3. 4.
M.J. Hÿtch, F. Houdellier, F. Hüe and E. Snoeck, Patent Application FR N° 07 06711. M. J. Hÿtch, E. Snoeck, and R. Kilaas, Ultramicroscopy 74 (1998), p. 131. F. Hüe, M.J. Hÿtch, H. Bender, F. Houdellier and A. Claverie, PRL (2008) accepted. F. Hüe is co-funded by the CEA-Leti. The authors thank the European Union for support through the projects PullNano (Pulling the limits of nanoCMOS electronics, IST: 026828)
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 5–6, DOI: 10.1007/978-3-540-85226-1_3, © Springer-Verlag Berlin Heidelberg 2008
6 and ESTEEM (Enabling Science and Technology for European Electron Microscopy, IP3: 0260019), and IMEC for the device material.
Figure 1. Bright-field image of an array of three dummy p-MOSFET strained-silicon channel transistors with Si80Ge20 sources and drains.
Figure 2. Experimental holographic dark-field: (a) hologram of (220) diffracted beam; (b) corresponding deformation map for εxx; (c) finite element modeling.
7
Some device challenges towards the 22nm CMOS technology F. Andrieu, T. Ernst, O. Faynot, V. Delaye, D. Lafond, S. Deleonibus CEA-LETI Minatec, 17 rue des Martyrs, 38054 Grenoble Cedex 9, France francois.andrieu@cea fr (invited abstract) Keywords: CMOS, integrated circuits
Since the 70’s, the transistor cost decreases exponentially thanks to the CMOS technology scaling down. However, this historical scaling is slowing down. Indeed, the IC’s manufacturers face different issues that the device engineers tend to solve thanks to a combination of both new materials and new architectures. The first (historical) challenge is to proceed the performance improvement while managing the dissipated power. Indeed, to achieve high performance devices, the supply voltage has not been reduced in the same proportion as the feature sizes. This has degraded the dynamic power consumption. The static power has increased even more [1]. At the same time, the performance enhancement has been limited by the difficult scaling of the gate oxide thickness (TOX). Strain has first been used, in order to maintain a good trade-off between performance and dissipated power. Stress Memorization Techniques, Nitride Contact Etch Stop Layers (CESL, see Figure 1), embedded SiGe source/drain [1] were integrated in the 65nm node. Moreover, wafer-level strain [2], (110) oriented substrates or Ge-based channels are currently evaluated in order to boost further the ON state currents of the sub-45nm technology. At the same time, new materials have been assessed to reduce the gate leakage. In particular, a combination of a Hf-based high-k dielectrics and a metal gate was introduced in the 45nm INTEL technology [3]. Finally, new architectures, like Fully Depleted thin films (planar, trigate or FINFETs) are evaluated as a solution to limit the source/drain leakage current (Figure 1-2) of sub-22nm devices. The second challenge is the scaling or, at least, the integration density growth, mainly because of the lithography limits. Moreover, even when the lithography techniques enable to draw aggressively scaled devices, it is found that strain is not necessarily as efficient as for longer ones. Finally, their OFF current is difficult to maintain because of the difficult scaling of all the other device dimensions (especially TOX and the junction depth). The historical scaling of the gate length thus tends to slow down. In the future, this trend will limit the integration density, unless new device architectures take over. Indeed, 3D layouts, like multi-channels or multi-fins structures already demonstrated very promising performance and density ([4], Figure 3-4). The third major concern is the variability issue. It is linked to the statistical technological variations (Line Edge Roughness of the gate, Random Dopant Fluctuation of the channel impurities…) that reduce the working window of the devices (e.g. the Static Noise Margin of the sub-45nm SRAM cells) [5]. To conclude, the slowing-down of the CMOS node shift (from 1.5 to 3 years per node) reflects 3 main technological issues: the more and more challenging trade-off S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 7–8, DOI: 10.1007/978-3-540-85226-1_4, © Springer-Verlag Berlin Heidelberg 2008
8
between performance enhancement and dissipated power, the difficult increase of the integration density and the variability issues. Microscopy techniques could help device engineers characterizing new materials and new architectures (where thin films are mandatory, cf. Fig.5 and [6]). However, to be relevant, they have to extract local information (about strain, doping, structure, compound, potential…) because the nanometer-range properties will govern the overall 22nm device performance and variability. 1. 2. 3. 4. 5. 6.
S.E. Thompson et al., IEEE Transactions on Electron Devices, 18, 1, p. 26, 2005. F. Andrieu et al., Micoelec. Eng. 84, p. 2047-53, 2007. K. Mistry et al., IEDM Tech. Dig., pp. 24750, 2007. T. Ernst et al., Proc. of ICICDT, 2008. F. Boeuf et al., VLSI Symp., pp. 24-5, 2007. V. Barral et al., IEDM Tech Dig., pp. 61-4, 2007.
TiN/HfO2
TiN/HfO2
20nm
CESL
9nm thin strained Si channel
Burried Oxide
Figure 1. TEM cross section in the electron transport direction of 25nm short FDSOI MOS with CESL and TiN/HfO2 (TSi=9nm). Si 3.4nm
9nm thin strained Si channel
Figure 2. TEM cross section perpendicularly to the electron transport direction of 40nm narrow FDSOI MOS with TiN/HfO2.
SiO2
4.8nm
Figure 3. Cross section of a silicon nanowire obtained by a self-limited oxidation to obtain a sub-5nm channel.
5nm
TiN HfO2
2 5nm thin strained Si channel
Figure 4. The 3D configuration of staked nanowires compensates the pitch-limited current density observed in planar trigate structures.
Figure 5. Integration of a 2.5nm thin strained Si channel MOS with very good performance [6].
9
Off-axis electron holography for the analysis of nm-scale semiconductor devices. D. Cooper1, R. Truche1, L. Clement2, S. Pokrant3, and A. Chabli1. 1. CEA LETI - Minatec, 17 rue des Martyrs, 38054 Grenoble, Cedex 9, France. 2. ST Microelectronics, 860 rue Jean Monnet, 38926 Crolles, France. 3. NXP Semiconductors, 860 rue Jean Monnet, 38926 Crolles, France. david.cooper@cea fr Keywords: off-axis electron holography, FIB, semiconductors
The reduction in the size of state-of-the-art semiconductors provides challenges for the characterisation of the doped regions during device development [1]. Off-axis electron holography is a promising TEM-based technique that can be used to provide 2D dopant maps with nm-scale resolution [2]. In this paper we will show how specimens containing nm-scale transistors are prepared using focused ion beam (FIB) milling for examination using off-axis electron holography. Parallel-sided specimens have been prepared using combinations of in situ lift out and back-side milling in order to avoid artefacts such as curtaining which can mask the phase measured in electrical junctions. Finally, low-energy FIB cleaning is used to reduce the thickness of the damaged surface regions on the specimens. Electron holograms have been acquired of state-of-the-art device specimens using a probe corrected FEI Titan electron microscope. The unprecedented electrical and mechanical stability of the Titan microscope allows electron holograms to be acquired for time periods of more than one minute allowing phase images of relatively thick, FIB prepared specimens to be reconstructed with a good signal-to-noise ratio [3]. Figure 1 shows reconstructed phase and amplitude images for a 45 nm gate nMOS device. In the amplitude image, no contrast is visible from the presence of the dopants, however, in the phase image the dopants can be clearly seen. The position of the gate is indicated by the white overlays. In this phase image, as well as the heavily doped regions (HDD), the lightly doped source and drain (LDD) regions can be clearly observed either side of the gate which can allow the electrical gate-width to be measured directly if all of the artefacts are understood. In this paper, we will discuss the suitability of using off-axis electron holography on FIB-prepared semiconductor specimens for dopant profiling. We will highlight many of the artefacts that are observed in phase images, including the effects of specimen thickness on the dopant concentration detection limit and the effects of strain in the doped regions. Finally we will show how electron holography has been applied to a range of samples in the semiconductor industry in order to support process development.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 9–10, DOI: 10.1007/978-3-540-85226-1_5, © Springer-Verlag Berlin Heidelberg 2008
10
1. 2. 3.
International Technology Roadmap for Semiconductors, 2005 ed. http://public.itrs net W.D. Rau, P. Schwander, F.H. Baumann, W. Hoppner and A. Ourmazd. Phys. Rev. Lett. 82, 2614 (1999). D. Cooper, R. Truche, P. Rivallin, J. Hartmann, F. Laugier, F. Bertin and A. Chabli. Appl. Phys. Lett. 91, 143501 (2007).
Figure 1. Shows a phase and amplitude image of a 450-nm-thick specimen prepared using FIB milling containing 45 nm gate nMOS devices.
11
Influence of the oxide thickness on the SiO2/Si interface structure P. Donnadieu1, V. Chamard2, M. Maret1, J.P. Simon1 and P. Mur3 1. SIMAP, INPGrenoble-CNRS-UJF, BP 75, 38402 Saint Martin d'Hères – France 2. IM2NP, CNRS - Université Paul Cézanne, 13397 Marseille Cedex 20 France 3. CEA-DRT-LETI-Minatec CEA-GRE 17 rue des Martyrs, 38054 Grenoble Cedex 9, France
[email protected] Keywords: Interface, HRTEM, geometric phase analysis, x-ray grazing incidence diffraction
A key issue in the elaboration of nanodots deposited on substrates is to be able to control their size, density and organisation. In that perspective, major attention has been given to monitor the substrate strain which may be helpful in some case to induce organization. In that context, we studied a currently used substrate: a Si wafer covered by an oxide layer. The typical thickness for such oxide layer is usually in the nanometer range : namely 1 to 10 nm. To characterize the structure and local chemistry of the oxide layer as well as the Si/oxide interface, TEM provides a large number of possibilities. X-ray surface sensitive techniques like Grazing Incidence Diffraction (GID) and reflectivity can also provide information on strain and electron density profile in the near surface region. We report here on a combined TEM and x-ray study carried out on a series of Si wafers covered with oxide layer of different thicknesses. HRTEM associated to the Geometrical Phase Analysis (GPA) method [1] was used to study the substrate deformation as a function of the oxide layer thickness. The samples were prepared by oxidation of 8 inch (100) CZ P type silicon wafers [2]. Prior to oxidation, the wafers are cleaned with an ozone based process. The oxides were elaborated, using a N2/O2 atmosphere at 800°C in a rapid thermal processing machine. According to ellipsometry measurement, the oxide thickness varies from 1.2 nm to 7 nm within the series we have studied. For each Si wafer, cross section samples have been prepared and examined by HRTEM. The images were further analysed by the GPA method. In the numerical analysis, the g(200) reciprocal vector has been selected to measure the displacement of the (200) planes, i.e. planes parallel the interface. Hence the phase map reported here displays the displacement component normal to the substrate surface. Figure 1a and 1b show a HRTEM image and the related GPA map. The profile in the insert gives the displacement as a function of the position along the AB line indicated in Figure 1b. There is a significant displacement in the vicinity of the surface (about 1-1.5 nm) while at distances larger than 1.5 nm, the almost flat profile indicates a negligible displacement. This behaviour has been observed for all samples, regardless of the oxide thickness between 1.2 and 7 nm. Figure 1c gives the measured displacement amplitude as a function of the oxide layer thickness. Error bars have been estimated from the fluctuations of repeated measurements on the phase maps.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 11–12, DOI: 10.1007/978-3-540-85226-1_6, © Springer-Verlag Berlin Heidelberg 2008
12
Figure 1. HRTEM image (Fig. 1a) and phase image for (200) g vector (Fig. 1b) (here the 1.2 nm oxide layer). In insert, the phase profile from A to B. Fig. 1c. plot of the total displacement as a function of thickness (the reported oxide thicknesses are measured by HRTEM which slightly differs from the ellipsometry ones). It comes out that the oxide layer thickness strongly influences the strain in the vicinity of the substrate (approximately 1-1.5 nm). Besides, for increasing thickness, larger displacement are measured (Figure 1c). In terms of deformation, it gives about 1 % for the 1.2 nm oxide thickness up to ~ 3 % for the 7 nm thickness. The relation between the oxide layer thickness and the deformation state of the substrate has been confirmed by observations on a two other samples : one with an extremely thin oxide layer (0.6 nm according to ellipsometry) and one with a thick oxide layer (80 nm). For the 0.6 nm oxide, GPA measurements were within error bars because of a too low strain. For the thick oxide layer, numerous dislocations were observed in the substrate close to the oxide layer which is consistent with the relaxation of a high level of strains. The x-ray GID measurement exhibits a 4-fold modulation of the oxide diffraction peak, which follows the Si[011] and the 3 other equivalent surface directions. This modulation, which shows the preferred orientation of the SiO4 tetrahedra at the interface, decays with increasing oxide thickness. Besides the analysis of x-ray reflectivity measurements emphasizes the presence of a dense interfacial layer (density mismatch ~ 8% for the 0.8 nm layer), which disappears with increasing oxide thickness. This combined TEM and X-ray study points out the complex structure of the oxide layer and the strain in the substrate at the vicinity of the interface. Both the oxide layer structure and the subtrate strain state are sensitive to the oxide thickness. It suggests that further nanostructure deposition may be influenced by the oxide layer thickness. This work has been carried out, in the frame of CEA-LETI / CPMA collaboration, with PLATO Organization teams and tools 1. 2. 3. 4.
M. J. Hytch, E. Snoeck, R. Kilaas, Ultramicroscopy 74, (1998) p. 131 P. Mur, M.-N. Semeria, M. Olivier, A.M. Papon, Ch. Leroux, G. Reimbold, P. Gentile, N. Magnea, T. Baron, R. Clerc, G Ghibaudo, Applied Surface Science 175-176 (2001) p. 726 M. Castro-Colin, W. Donner, S. C. Moss, Z. Islam, S. K. Sinha, R. Nemanich, H. T. Metzger, P. Bösecke and T. Shülli, Phys. Rev. B 71, (2005) p. 045310. We kindly acknowledge the ESRF for allocating beamtime and the ESRF ID1 staff for their help during x-ray experiments.
13
Challenges to TEM in high performance microprocessor manufacturing H.J. Engelmann, H. Geisler, R. Huebner, P. Potapov, D. Utess, E. Zschech AMD Saxony LLC & Co. KG, CCA, MS E23-MA, D-01109 Dresden, Germany
[email protected] Keywords: Electron Tomography, EELS, Strain Analysis, Dark-Field Diffraction
Smaller structures and new materials require the application of advanced TEM techniques for process control and failure analysis in 45 nm CMOS technology node and beyond. Both imaging TEM and analytical TEM techniques have to be modified or adapted to special questions. There are several reasons for that: A) Device structures that have to be characterized are often located completely within a TEM lamella. For example, typical gate lengths of 45 nm technology node transistors are in the range between 40 and 45 nm. The diameters of respective contacts are smaller than 80 nm. Assuming a standard lamella thickness of 60…80 nm, not all details of a 3D structure can be seen in the 2D projection image anymore. A possible approach to solve this problem is the application of Electron Tomography. While tomographic image acquisition and data treatment have already become a standard technique, sample preparation is still a challenge, especially in case of failure analysis. As an example, Figure 1 shows the 3D reconstruction of a defect in the contact area. Missing silicide caused an increased electrical resistance in that case. B) The application of new materials requires the characterization of their properties in dependence on deposition and treatment parameters. For example, low-k dielectric materials which are used to reduce the cross-talk between Cu interconnects show changes in chemical composition caused by plasma etch processes. The resulting kvalue increase has to be measured in the direct neighbourhood of etched structures like trenches and vias, with a spatial resolution better than 5 nm. While changes in chemical composition are analyzed by EELS, direct measurement of the k-value can be done by Valence EELS. A procedure was developed which allows determining the 1014 Hzfrequency dielectric permittivity [1]. Even though this is not the k-value corresponding to the GHz-frequency range used in microprocessors, relative changes in the dielectric constant can be detected very precisely (Figure 2). Ultra low-k (ULK) materials that are expected to be introduced for the 32 nm CMOS technology node will contain pores. Local pore size/pore distribution characterization will be another challenge for TEM. C) The introduction of ‘strained silicon’ into the channel region of transistors requires advanced characterization techniques. Mechanical stress results in a distortion of the silicon lattice which affects the electronic band structure, allowing improvements in carrier mobility. For process control and next technology node transistor development, local strain measurements in the Si MOSFET channel are needed. Nano Beam Diffraction (NBD) is an analysis technique that uses a small probe electron beam with reduced convergence angle to produce diffraction patterns with smaller spots than in CBED patterns [2]. The lattice parameter can be determined from the positions of the S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 13–14, DOI: 10.1007/978-3-540-85226-1_7, © Springer-Verlag Berlin Heidelberg 2008
14
spots which allows strain quantification. The challenge in this technique is the NBD pattern analysis for very precise lattice spacing determination which is needed for strain quantification. Figure 3 shows the relative change of the Si lattice spacing in <110> direction in the channel region of a tensile strained NMOS transistor. D) With shrinking of structure sizes new questions arise regarding product reliability. For example, the Cu microstructure becomes more and more important with decreasing dimensions of the interconnect lines. Grain size, grain orientation and twin formation can influence the stability against electromigration/stress migration to a high degree. So far, the EBSD technique has been used to characterize the Cu microstructure. Since agglomerates of small Cu grains are expected to be a reliability concern for the 32 nm CMOS technology, grains with sizes below 40 nm have to be analyzed which requires a TEM-based technique. Dark-Field Diffraction Circular Scanning with subsequent diffraction pattern reconstruction can be used to produce grain orientation maps. As an example, Figure 4 shows a [001] inverse pole figure map of a Cu interconnect stack. Further challenges exist in the field of sample preparation: Quality/precision, target preparation for failure analysis/defects and sample throughput. 1. 2. 3.
P. Potapov, H.J. Engelmann, E. Zschech, M. Stöger-Pollach, submitted to Micron. H.J. Engelmann, S. Heinemann, E. Zschech, Proc., IMC 16, Sapporo, Sept. 3-8, 2006. We kindly acknowledge the financial support by the German BMBF, FKZ 13N9431
Figure 1. 3D reconstruction of a defect in the contact area
Figure 2. Relative change in dielectric constant in surface-plasma treated low-k material (covered with a Cr layer).
Figure 3. Relative change of Si lattice spacing in NMOS channel region
Figure 4. Inverse pole figure map of a Cu interconnect stack
15
Strain study in transistors with SiC and SiGe source and drain by STEM nano beam diffraction P. Favia1, D. Klenov2, G. Eneman1,3, P. Verheyen1, M. Bauer4, D. Weeks4, S.G. Thomas4 and H. Bender1 1. IMEC, Kapeldreef 75, 3001 Leuven, Belgium 2. FEI, Achtseweg Noord 5, 5651 GG Eindhoven, The Netherlands 3. K U Leuven, ESAT/INSYS, and Fund for Scientific Research-Flanders, Belgium 4. ASM America, 3440 E. University Dr., Phoenix, AZ 85034, USA paola
[email protected] Keywords: nano-beam diffraction, strain, SiGe, SiC
Strain is introduced in the fabrication of complementary metal-oxide-semiconductor devices to enhance their channel region carrier mobility [1]. Epitaxial Si1-xGex (1530at% Ge) or Si1-xCx (1-2at% C) are typical stressor materials. As Ge has a 4% larger lattice constant (0.566 nm) than Si (0.543 nm), Si1-xGex deposited in the source/drain (S/D) regions will induce compressive strain in the Si channel, while Si1-xCx in the S/D will induce tensile strain in the channel [2]. Nano-beam diffraction (NBD) is a TEM-based technique that allows to obtain a diffraction pattern from small regions and, as a result, to measure directly local lattice parameter and thus to quantify 2-D strain. NBD uses a small diameter electron probe which determines the lateral resolution (<10 nm) and which has a small convergence angle so that the diffraction patterns show sharp spots. To obtain this condition, a small condenser aperture (10 μm) is used in microprobe STEM mode in a Tecnai F30. Two series of transistors, having Si80Ge20 and Si99C1 S/D respectively and different channel lengths were investigated. These epitaxial layers were grown using an ASM Epsilon® 2000 reactor. TEM specimens were prepared by focused ion beam for [1-10] zone axis observation. Series of electron diffraction patterns were acquired in the channel region perpendicular to the gate (Figure 1). Data were processed using the FEI True Crystal Strain software which automatically determines the center of the diffraction spots and calculates the displacement of their positions with respect to the reference diffraction pattern. Strain variations in the horizontal [110] and perpendicular [001] (growth) direction, were obtained along a line profile perpendicular to the interface. Experimental data were converted from strain to stress and then compared with simulations performed by the finite-element simulator Taurus-Process by Synopsys [3]. Figure 2 shows the horizontal strain variation measured perpendicular to the interface in channels having on mask lengths 500nm, 250nm and 90nm respectively and 250nm wide Si1-xCx S/D. As expected Si1-xCx induces channel tension. The strain is smaller (0-0.2%) in larger channels and reaches higher values of about 0.5% in the 90nm channel. The strained region extends deeper in the Si substrate as the channel length is reduced.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 15–16, DOI: 10.1007/978-3-540-85226-1_8, © Springer-Verlag Berlin Heidelberg 2008
16
Figure 3 shows the horizontal experimental and simulated stress variation perpendicular to the interface in structures having Si channels and Si1-xGex S/D. In these devices the stress is, as expected, compressive in the channel along the [110] direction. Measured stress is in good agreement with the simulated one. Table 1 shows a summary of the experimental results for maximum strain and depth of strain penetration in the Si substrate as a function of the gate length for the two types of investigated devices. In general, the shorter the gate, the larger is the strain (either compressive or tensile) and the deeper is the penetration in the Si substrate. The results obtained in this work by NBD are fairly consistent with theory and simulations, proving that the NBD technique can be reliably applied to such structures. 1. 2. 3.
B. Foran, M. H. Clark and G. Lian, Future Fab International 20 (2006), p. 127. N. Bich Yen, V. Vartanian, A. Thean, et al., Solid State Technology 49 (2006), p. 41. Taurus TSUPREM, Taurus Process Reference Manual, Oct. 2005. Version X-2005.10. a
b
transistor SiC
transistor
SiGe
SiC
SiGe
lineprofile [001]
Si
100 nm
lineprofile
100 nm
[110]
Si
Figure 1. HAADF image of a transistor with SiC (a) and SiGe (b) S/D. 0.8
0.4
0.0
0.8
L/S=250nm/250nm Strain (%)
L/S=500nm/250nm Strain (%)
Strain (%)
0.8
0.4
0.0
-0.4
-0.4 0
100
200
300
400
0.0
-0.4 0
500
L/S=90nm/250nm
0.4
100
200
300
400
500
0
100
Distance (nm)
Distance (nm)
200
300
400
500
Distance (nm)
Figure 2. Tensile strain along [110] in SiC S/D transistors. The lineprofile is perpendicular to the interface under the gate (Figure 1).
-1 -2
1
L/S=130nm/250nm
0 -1 -2 -3
-3 0
100
200
300
400
Distance (nm)
1 Stress (GPa)
L/S=200nm/250nm
0
Stress (GPa)
Stress (GPa)
1
L/S=100nm/250nm
0 -1 -2 -3
0
100
200
300
400
Distance (nm)
0
100
200
300
400
Distance (nm)
Figure 3. Experimental (marker) and simulated (line) stress along [110] in Si channels with SiGe S/D. The lineprofile is perpendicular to the interface (Figure 1). Table I S/D SiC SiC SiC SiGe SiGe SiGe
On mask gate length (nm) 500 250 90 200 130 100
Max perpendicular strain (%) 0.1 0.3 0.5 -0.8 -1.3 -1.8
Strain penetration in the Si (nm) 40 90 130 150 100 100
17
Cluster growth and luminescence in ion-implanted silica H.-J. Fitting1, Roushdey Salh1, L. Kourkoutis2, and B. Schmidt3 1. Physics Dept., Rostock University, Universitaetsplatz 3, D-18051 Rostock, Germany 2. Applied and Engineering Physics, Cornell University, Ithaca NY 14853, U.S.A. 3. Institute of Ion Beam Physics, Res. Center Dresden-Rossendorf, D-01314 Dresden, Germany hans-joachim
[email protected] Keywords: Cathodoluminescence, Silica layers, Ion implantation
Scanning electron microscopy (SEM) and cathodoluminescence (CL) in combination with scanning transmission electron microscopy (STEM) have been used to investigate thermally grown amorphous silicon dioxide layers implanted isoelectronically with group IV ions (C+, Si+, Ge+, Sn+, Pb+) as well as with group VI ions (O+, S+, Se+), see Fig.1. As the main experimental results we can state: Oxygen surplus increases the red band (R) in SiO2 but does not affect the blue band (B). Silicon surplus increases the blue luminescence B, but reduces the red band (R) as already demonstrated in [1]. So it is verified that the red luminescence (R) is an oxygen related center stated as NBOHC and the blue luminescence (B) is a silicon related oxygen deficient center Si-ODC. In Ge+ implanted SiO2 a strong violet band V (3.1 eV ; 410 nm) appears and is associated with the Ge-related oxygen deficient center Ge-ODC. This V band shows a huge increase after thermal annealing of Ta=900 °C by more than two orders of magnitude. Thus the Si-ODC's as well as the Ge-ODC's are formed by Si and Ge molecules clustering to certain low-dimension fragments like dimers ODC-I, trimers and up to higher aggregates, [2]. The nanocluster size grows with annealing temperature from 2-4 nm at Ta=900 °C to 5-10 nm at Ta=1100 °C, see e.g. Fig. 2. Further ion implantations of group IV elements: C, Ge, Sn, Pb which are thought to substitute Si isoelectronically in the silica matrix, show new bands and a general increase of the luminescence in the violet-blue region. On the other hand, implantations of oxygen substituting elements of group VI (S, Se) lead to an increase in the yellow-red spectral region, [2]. As a surprising peculiarity, the cathodoluminescence spectra of the group VI elements oxygen and sulfur implanted SiO2 layers show, besides characteristic bands, a sharp and intensive multimodal structure as shown in Fig. 3. The energy step differences of the sublevels amount to an average of 120 meV and indicate vibronicelectronic transitions, probably, of O2− interstitial molecules, as we could demonstrate by a respective configuration coordinate model, [3]. 1. 2.
H.-J. Fitting, T. Barfels, A. N. Trukhin, B. Schmidt, A. Gulans, and A. von Czarnowski, J. Non-Cryst. Solids 303 (2002) 218 – 231. Roushdey Salh, L. Fitting-Kourkoutis, B. Schmidt, H.-J. Fitting, Physica Status Solidi (a) 204 (2007) 3132 – 3144
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 17–18, DOI: 10.1007/978-3-540-85226-1_9, © Springer-Verlag Berlin Heidelberg 2008
18 3.
H.-J. Fitting, Roushdey Salh, T. Barfels, and B. Schmidt, Physica Status Solidi (a) 202 (2005) R142 – R144. 80
SiO2
Eo=1 keV
Si
SiO2
Si
60 50
Ge 40
3 keV 4 keV 5 keV 6 keV 8 keV
30 20
10 keV
12 keV
15 keV
30 keV
0
surface
100
200
300 Rp
400
depth (nm)
500 interface
Ge
25 keV
10 0
interface
2 keV
surface
energy transfer (eV/nm)
70
600 substrate
100 nm
700
Ge+ implantation profile
Figure 1. Electron beam excitation in SiO2 layers for different beam energies Eo allowing a CL depth profiling (left). Here a Ge profile is implanted in the mean projected range Rp ≈250 nm. The STEM micrograph (contrast inverted) shows the actual Ge cluster profile.
Figure 2. Ge cluster growth in silica with increasing annealing temperatures Ta, (Ostwald ripening).
Figure 3. Multimodal CL spectra from sulfur-implanted SiO2:S layers, recorded at liquid nitrogen temperature (LNT).
19
Coherence Measurements of Bulk and Surface Plasmons in Semiconductors by Diffracted Beam Holography R.A. Herring Center for Advanced Materials & Related Technologies, Mechanical Engineering, University of Victoria, Victoria Canada V8W 3P6
[email protected] Keywords: plasmon loss electrons, electron holography, coherence
The degree of coherence (γ) and lateral coherence (δ) of plasmon loss electrons has been measured using two methods of energy-filtered Diffracted Beam Interferometry/Holography (DBI/H); one using high-angle scattered electrons produced by a small probe of a few Angstroms referred to as convergent DBI/H [1] and another one using a variable, large-diameter planar beam referred to as planar DBI/H [2] (Figure 1). Both DBI/H methods require a (S)TEM with an electron source having good coherence, an electron biprism for holography and an imaging energy filter (GIF) for separating out the plasmon loss electrons. Surface and bulk plasmon excitations are created by the fast electron during its passage into and through the material specimen. After the creation event, these plasmon loss electrons retain all of the plasmon’s coherence information. An important consideration in these measurements is dynamic diffraction, which is accounted for in the simulations of energy-filtered convergent DBI/H by use of the mixed dynamic form factor [5]. To help reduce dynamic diffraction, thin specimens of ~¼ extinction distance of the diffracted beam (~15 nm) have been used, which also produces equal intensity beams that provide for the highest contrast fringes and simplifies the measurement of γ and δ. Additionally, convergent DBI/H uses the condenser aperture focused on the diffraction plane for separating out the source electrons from the plasmon loss electrons at large scattering angles (Figure 2). A γ of ~0.1 was measured at scattering angle of ~ 7 mrad. The fringes disappeared when the interfering beams were separated using the electron biprism from the exact overlay position, which has produced measurements of the lateral coherence of ~1 nm on the specimen plane. It is believed that the surface plasmon loss electrons dominate the energy-filtered electron intensity at large beam diameters. As the planar beam diameter becomes larger in planar DBI/H, the surface plasmons lose their mutual coherence resulting in a decrease and eventual loss of their fringe contrast in the center of the interferogram giving a measurement of δ (Figure 3). Knowledge of δ of bulk plasmons and surface plasmons would be very helpful for understanding nanoscience and for developing nanotechnology. 1. 2. 3.
R.A. Herring, Ultramicroscopy 104 (2005) 261. R.A. Herring, Ultramicroscopy (2007). In press. P. Schattschneider and J. Verbeeck, Ultramicroscopy (2007). In press.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 19–20, DOI: 10.1007/978-3-540-85226-1_10, © Springer-Verlag Berlin Heidelberg 2008
20 4.
FEI, Eindhoven and CEMES, Toulouse are gratefully acknowledged for the use of their microscopes. Grants from UVic, NSERC and the CFI are also gratefully appreciated.
a) b) Figure 1. Schematics showing convergent DBI/H in a), an amplitude splitting method with no interference of the beams and biprism, and planar DBI/H in b), a mixed amplitude plus wavefront spitting method having beam and biprism interference.
a)
c) b) Figure 2. Energy-filtered convergent DBI/H of plasmon loss electrons of Ge showing an over-exposed hologram in a), intensity profile extending away from center along white line in b), and retained coherence of high-angle scattered electrons in c).
γ = 0.2
d) a) c) Figure 3. Energy-filtered convergent DBI/H of plasmon loss electrons of Ge (in a) and b)) and of Si (in c) showing a hologram at position 1 in Fig 2a using a small electron probe of a few Å in a), and planar DBI/H holograms in b) using 200 nm diameter beam and in c) using 2000 nm diameter beam, giving δ ~ 2000 nm for Si.
21
Comparison of 3D potential structures at different pn-junctions in FIB-prepared silicon and germanium samples measured by electron-holographic tomography A. Lenk1, D. Wolf1, H. Lichte1 and U. Mühle2 1. Triebenberg Laboratory, Institute of Structure Physics, Technische Universität Dresden, D-01062 Dresden, Germany 2. Qimonda Dresden GmbH & Co. OHG, Königsbrücker Straße 180, D-01099 Dresden, Germany
[email protected] Keywords: p-n junction, intrinsic electrostatic potential, specimen surface
The functionality of electronic nanodevices is essentially determined by location, extension and concentration of the enclosed doped areas. Therefore, the manufacturing of those areas is one of the most important tasks in semiconductor industry. In general, it consists of two steps: First, the dopant material has to be inserted into the lowly doped semiconductor substrate. Then, the inserted dopants have to become electrically activated. Electron holography allows to monitor the outcome of both processes simultanously by providing 2D mapping of the resulting electrostatic potential distribution in the semiconductor [1]. Though, prerequisite for such an analysis is an appropriate preparation method. Precise target preparation, needed for the very small semiconductor devices, leaves no alternative to the application of a Focussed-Ion-Beam (FIB) tool. It has been shown that the method can be adapted to the special requirements of electron holography [2]. Unfortunately, the FIB-treatment always alters the electrical and structural characteristics of the sample, or at least those of the micromachined lateral surfaces and their adjacent regions. For a successful quantitative evaluation of the measured data, this has to be understood and taken into account. For this purpose, a new needle-shaped specimen geometry (shown in Figure 1) was designed and used to investigate a conventionally FIB-prepared lamella in cross-section [3]. Such needles are also highly qualified for tomographic application in the TEM. So it was possible to measure and compare 3D distributions of the electrostatic potential in silicon needle samples with pn-junctions of both types. Figure 2a/b shows a comparison of two virtual slices through the inner core of reconstructed 3D needles. It was found out, that the potential ascend in n-doped areas surrounded by p-doped substrate (0.44 V in Figure 2a) is smaller then the potential descend in p-doped regions surrounded by ndoped substrate (0.92 V in Figure 2b) [4]. In theory, both differences should be equal. To investigate this effect further, a germanium-based needle with an n-doped top layer has been analysed with electron holography, conventionally and tomographically. Figure 2c shows the holographically measured potential shift at the germanium pnjunction. Again, the measured potential drop ist lower than theoretically expected.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 21–22, DOI: 10.1007/978-3-540-85226-1_11, © Springer-Verlag Berlin Heidelberg 2008
22
1. 2. 3. 4.
W.-D. Rau, P. Schwander, F. H. Baumann, W. Höppner, and A. Ourmazd, Physical Review Letter 82 (1999), p. 2614. A. Lenk, H. Lichte and U. Mühle, Journal of Electron Microscopy 54(4) (2005), p. 351. A. Lenk, U. Mühle and H. Lichte, Springer Conference Series “Microscopy of Semiconducting Materials XIV”(2005), p. 213. A. Lenk, D. Wolf and U. Mühle, Conference Proceedings of MC Saarbrücken (2007), p. 306.
Figure 1: Images of a needle-shaped specimen. Left: Top view in the FIB after cutting. Right: Bright field image in a TEM. Because of its special symmetric geometry, the needle can be used as a cross-section of a conventionally FIB-prepared lamella.
Figure 2. Holographically measured potential differences at different pn-junctions in silicon and germanium samples. 2a: n-doped layer in p-doped silicon. 2b: p-doped layer on n-doped silicon. 2c: n-doped layer on p-doped germanium. The images 2a & 2b are slices from tomographically reconstructed virtual needles, whereas image 2c is a phase image from a conventionally recorded hologram.
23
EELS analyses of metal-inserted high-k dielectric stacks M. MacKenzie1, A.J. Craven1, D.W. McComb2, C.M. McGilvery2, S. McFadzean1 and S. De Gendt3 1. Department of Physics & Astronomy, University of Glasgow, Glasgow, G12 8QQ, UK 2. Department of Materials, Imperial College London, London, SW7 2AZ, UK 3. IMEC, Kapeldreef 75, B-3001 Leuven, Belgium. Also at KU Leuven, B-3001 Leuven, Belgium
[email protected] Keywords: high-k dielectric, metal gate, EELS, ELNES
Hf-based systems are going into production this year as the high-k materials replacing amorphous SiO2 and Si(O,N) as the gate dielectric in Si MOSFETs. At the same time, metal inserted poly-Si gate electrodes are being used in the gate stacks to remove problems associated with poly-Si gate electrodes. Significant interface interactions can occur in such systems as a result of the thermal budget received during device processing. We are investigating a range of HfO2 and HfSiO based stacks with TiN or TaN metal inserted poly gates. The effect of different deposition methods and processing treatments on physical and chemical properties are probed via electron energy loss spectroscopy (EELS). In particular, interface reactions occurring between the layers in the stack are investigated using the electron energy loss near edge structure (ELNES) to extract information on the phases present. The specimens are examined in an FEI Tecnai F20 TEM/STEM equipped with a field emission gun, a Gatan ENFINA electron spectrometer and an EDAX X-ray spectrometer. Spectrum imaging was performed using Gatan DigiScan II and Digital Micrograph software. Mounted on one of the 35 mm camera ports is a retractable fast beam switch (FBS) [1,2]. The FBS allows us to collect the EELS core and low loss spectra from the same regions under the same electron-optical conditions and hence to remove the effects of plural scattering and normalize the overall signal level. Absolute elemental quantification is thus enabled. Figure 1(a) shows a high resolution TEM image of a Si/SiO2/HfSiO/TaN/poly-Si gate stack. As well as an amorphous phase at the TaN/poly-Si interface, one can observe lighter patches in the TaN layer. The high angle annular dark field (HAADF) STEM image of the same stack in Figure 1(b) shows dark notches penetrating into the TaN from the TaN/poly-Si interface. We have previously reported some EELS results across this stack and shown the presence of an oxide phase at the TaN/poly-Si [3]. Here we investigate the dark notches in the HAADF STEM images. An EELS spectrum image was acquired across one of these notches along the white line in Figure 1(b). Figure 2(a) contains the N and O elemental profiles obtained from the spectrum image and shows that the dark notch corresponds to an oxidised region of TaN. The
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 23–24, DOI: 10.1007/978-3-540-85226-1_12, © Springer-Verlag Berlin Heidelberg 2008
24
background subtracted O K-edge part of the spectrum image shown in Figure 2(b) also confirms this.
(a)
poly -Si
TaN
Si
(b) Si
poly-Si
SiO2 HfSiO
HfSiO
TaN
50 nm
5 nm
(a)
(b) N O
0
10
20 distance (nm)
30
distance (nm)
Intensity (arbitrary units)
Figure 1. (a) High-resolution TEM image of a Si/SiO2/HfSiO/TaN/poly-Si gate stack. (b) HAADF STEM image of a Si/SiO2/HfSiO/TaN/poly-Si gate stack. An EELS spectrum image dataset was acquired across the gate stack as indicated by the white line.
Energy Loss (eV)
Figure 2. (a) N and O elemental profiles extracted from an EELS spectrum image acquired along the line shown in Fig. 1(b); the substrate is on the LHS. (b) Background subtracted O K-edge spectrum image. The Si substrate is at the top. 1. 2. 3. 4.
A.J. Craven, J. Wilson and W.A.P. Nicholson, Ultramicroscopy 92 (2002), p. 165. J. Scott, P.J. Thomas, M. MacKenzie, S. McFadzean, J. Wilbrink, A.J. Craven and W.A.P. Nicholson, submitted to Ultramicroscopy (2008). M. MacKenzie, A.J. Craven, D.W. McComb, C.M. McGilvery, S. McFadzean and S. De Gendt, submitted to proceedings of MSMXV 2007, Cambridge. We kindly acknowledge the EPSRC for funding (GR/S44280) and B. Miller (University of Glasgow) for TEM specimen preparation.
25
Low voltage SEM observations of the dopant contrast in semiconductors K. Masenelli-Varlot1, S. Luca1, G. Thollet1, P.H. Jouneau2 and D. Mariolle3 1. Université de Lyon, MATEIS UMR 5510, INSA-Lyon, 7 avenue Jean Capelle, 69621 Villeurbanne, France 2. CEA/INAC/SP2M/LEMMA, 17 avenue des Martyrs, 38054 Grenoble, France 3. CEA/LETI, 17 avenue des Martyrs, 38054 Grenoble, France karine-masenelli.varlot@insa-lyon fr Keywords: semiconductor, SEM, doping contrast
The electrical properties and performances of most semiconductor devices depend on their dopant concentration. For this reason the Semiconductor Industry needs a twoand three-dimensional dopant profiling technique with nanometric spatial resolution in the range of sensitivity between 1016 and 1020 atm/cm3 and an accuracy of ±10%. One of the few 2D dopant profiling technique that can fulfil these requirements is the scanning electron microscopy (SEM), which is a fast and non-destructive technique, with a rapid sample preparation. However it was shown that it has some limitations because of the lack of reproducibility in the image acquisition [1]. In this paper we present a study on the doping contrast in Si semiconductor structures by Low Voltage Scanning Electron Microscopy (LVSEM). The experiments were performed on low vacuum FEG-SEM Zeiss Ultra55 and FEI XL 30 ESEM. The particularity of the last one is that it can work either in HV or under a gas pressure. The advantage of using the gaseous environment is that positive ions, created by interactions between the incident electrons and gas molecules, neutralize the charges accumulated at the sample surface [2]. Several p-doped Si multilayers with dopant concentrations from 2·1017 atm/cm3 to 3·1019 atm/cm3, elaborated by RP-CVD, were investigated. The SIMS profile and the LVSEM image of a sample is given in Figure 1. One can clearly distinguish the difference in contrast between the five doped layers. As mentioned in the literature [1], the doping contrast is substantially affected by the surface quality (oxidizing, contamination, …) and by several experimental parameters (scan time, magnification, accelerating voltage, …). Indeed after a few minutes of investigation, we detect a decrease of the contrast. At lower magnification, the formation of a “window” can be observed in the region scanned previously (Figure 2). This phenomenon was already presented in the literature as a contamination effect [3] but it also can be due to charges accumulated at the surface of the sample. In order to have no contrast decrease and thus obtain a good reproducibility, we developed a procedure for the sample preparation and observation, which includes in situ decontamination of the sample. Using that procedure, reproducible images can be obtained and the quantification of the dopant level can be performed with a good accuracy.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 25–26, DOI: 10.1007/978-3-540-85226-1_13, © Springer-Verlag Berlin Heidelberg 2008
26
Figure 1. SIMS profile and LVSEM observation on a p-doped Si multilayer structure. The SEM image was made on the Zeiss Ultra55 at 1 kV and WD = 3 mm in HV.
Figure 2. LVSEM image on the same sample at lower magnification, in HV. 1. 2. 3.
P. Kazemian, C. Rodenburg, C.J. Humphreys, Microelectronic Engineering 73-74 (2004), 948-953. A.M. Donald, Nature Materials 2 (2003), 511-516. W.H. Bruenger, H. Kleinschmidt, W. Hässler-Grohne, H. Bosse, J. Vac. Sci. Technol. B15 no. 6 (1997), 2181-2184.
27
NiSi2/Si interface chemistry and epitaxial growth mode S.B. Mi1, C.L. Jia1, K. Urban1, Q.T. Zhao2, and S. Mantl2 1.Institute of Solid State Research and Ernst Ruska-Centre for Microscopy and Spectroscopy with Electrons (ER-C), Research Centre Juelich, D-52425 Juelich, Germany 2.Institute of Bio- and Nanosystems (IBN1), and Center of Nanoelectronic Systems for Information Technology (CNI), Forschungszentrum Jülich GmbH, D-52425 Jülich, Germany s
[email protected] Keywords: Interface, Microstructure, Transmission Electron Microscopy
In recent years, lots of efforts have been contributed to produce epitaxial thin films of transition metal silicides on silicon substrate for fundamental studies on electrical and structural properties of interface, as well as for application as Schottky and ohmic contacts on silicon-based devices [1-3]. Since the electronic properties in metal/semiconductor junctions strongly depend on the interface structure, i.e., coordination of metal atoms, reconstruction and defects at the interface, it is of great interest to exploring the atomic structure of the interface. In this work, NiSi2 thin films are formed by annealing a Ni film deposited on a sulfur implanted-silicon (100) wafer [4]. With Surfer, which can tune the Schottky barrier height of NiSi/Si contacts [5], the interface in the NiSi2/Si system brings an additional interest of research. The atomic structure and chemistry of the NiSi2/Si interface are investigated by means of aberration-corrected transmission electron microscopy. The films grow epitaxially with an atomically sharp interface defined mainly of the (100) plane with a few {111} facets. At the (100) interface, 5-coordinated Si atoms facing 7-coordinated Ni atoms, form a 2 × 1 reconstruction structure. At the {111} facets, Ni atoms are remain to be 7-coordinated while Si atoms are 4-coordinated as in bulk. Interfacial dislocations with Burgers vectors a/4<111> and a/2<110> are observed near {111} facets with the extra half atomic planes in the Si substrate, which is the reverse of what happen between bulk NiSi2 and Si. This novel phenomenon can be understood in the light of growth modes of NiSi2 thin films with a high concentration of S at the interface. 1. 2. 3. 4. 5.
R.T. Tung,J.M. Gibson,J.M. Poate, Phys. Rev. Lett. 50 (1983) 429-432. H. von Känel, Mater. Sci. Reps 8 (1992) 193-269. C. Schwarz, H. von Känel, J. Appl. Phys. 79 (1996) 8798-8807. Q.T. Zhao, S.B. Mi, C.L. Jia, U. Breuer, S. Lenk, S. Mantl, et al., to be submitted Q.T. Zhao, U. Breuer, E. Rije, St. Lenk, S. Mant, Appl. Phys. Lett. 86 (2005) 062108.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 27–28, DOI: 10.1007/978-3-540-85226-1_14, © Springer-Verlag Berlin Heidelberg 2008
28
Figure 1 A cross-sectional low-magnification TEM image of NiSi2/Si viewed along the <011> zone axis. The (100) interface is indicated by a horizontal arrow. {111} facets are indicated by vertical arrows.
29
Detailed investigation of a tunnel oxide defect in a flash memory cell using TEM-tomography U. Muehle1, M. Krause1, F. Goetze2, D. Wolf 3, and U. Gaebler4 1. Qimonda Dresden GmbH & Co. OHG, Koenigsbruecker Str. 180, D-01099 Dresden, Germany 2. Institute of Material Science, TU Dresden, D-01062 Dresden, Germany 3. Triebenberg Laboratory, ISP, TU Dresden, D-01062 Dresden, Germany 4. Infineon Dresden GmbH & Co. OHG, Koenigsbruecker Str. 180, D-01099 Dresden, Germany
[email protected] Keywords: tomography, flash memory cell, gate oxide
TEM-investigations are of increasing relevance for process monitoring and physical failure analysis in semiconductors industry [1]. However, due to decreasing dimensions of structural elements a situation can be predicted, where the details to be observed are smaller than the thickness of TEM-foil, prepared by the usual FIB-technique for target preparation [2]. Furthermore, several issues of failure analysis are limited in electrical methods for localisation, leading to an uncertainty about the optimised location of the final specimen. Therefore TEM-tomography might be able to localise and characterise the physical reason of an electrical failure by reconstruction up a 3D-model. [3] In the present case a flash memory cell showed a charge loss, probably caused by an anomaly at the active silicon surface or in the tunnel oxide. A primary investigation was performed at a TEM-foil with a thickness of more than 150 nm, including the whole width of the cell (Figure 1a). The TEM bright field image contained a suspicious detail, as shown in the close up view (Figure 1b), leading to the assumption of a so called “pit” in the surface of silicon. The comparison of its dimension to foil thickness explains the poor contrast behaviour. Further reduction of foil thickness by FIB is risky, because no information about the defect location over the foil thickness is available. For tomographic investigation a rearrangement of the sample for realisation of high tilt angles is required. In order to achieve tilt angles as high as possible, the sample was rearranged using in-situ lift-out technique [4]. The free standing sample allowed the acquisition of a tilt series from -65° till +65° using HAADF-STEM to reduce dynamic effect of the crystalline materials. The investigation was done in a Tecnai F20, equipped with a tomography samples holder type “Fischione 2020”. For data acquisition and reconstruction the FEI software-packet of Explore3D/Inspec3D was used. [5] The defect can easily be identified by slicing through the reconstructed 3D-volume. Location in any direction, lateral dimension and depth of the “pit” can be determined (Figure 2). The comparison with results of the electrical test leads to conclusions, how to avoid the this kind of defects or to guarantee a successful coverage by testing.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 29–30, DOI: 10.1007/978-3-540-85226-1_15, © Springer-Verlag Berlin Heidelberg 2008
30 1. 2. 3. 4. 5.
Vallett, D.P.; IEEE Transact. 1 (2002); p. 117-121 http://www future-fab.com/documents.asp?d_ID=3004 Kubel, C., Kubel, J., Kujawa, S., Luo, J.S., Lo, H.M., Russell, J.D.; 8th Int. Works. on Stress-Induced Phenomena in Metallization, AIP Conf. Proc., Vol. 817, (2006), pp. 223-228 http://www.omniprobe.com/pdf/sp1.pdf Tomography acquisition and reconstruction guide; FEI-company; Manual
Figure 1. Overview of a failing flash memory cell (a-left side) and suspicious detail with poor contrast (b-right side) in TEM-bright field.
Figure 2. Virtual slicing through the 3D-model in the plane of the “pit” in two directions.
31
Overgrowth of the Mn4Si7 phase on/around the hexagonal SiC and cubic MnSi impurity phases in the Mn4Si7/Si films A. Orekhov1, T. Kamilov2 and E.I. Suvorova1,3 1. A.V. Shubnikov Institute of Crystallography of Russian Academy of Sciences, Moscow, Russia 2. Tashkent State Aeronautical Institute, Uzbekistan 3. CIME, Ecole Polytechnique Fédérale de Lausanne, Lausanne, Switzerland
[email protected] Keywords: Mn4Si7/Si films, impurity phases, TEM and X-ray EDS analysis
Structural and morphological analysis of Mn4Si7 films using the TEM/HRTEM/ Electron diffraction/STEM/EDS modes in a FEI CM300UT FEG electron microscope was carried out in a FEI CM300UT FEG electron microscope in TEM/HRTEM/ Electron diffraction/STEM/EDS mode. The images were recorded on a Gatan 797 slow scan CCD camera and processed with the Gatan Digital Micrograph 3.11.1 software, INCA (Oxford) and JEMS package [1]. The preparation of the films was performed by solid phase reaction during the evaporation of the resublimed Mn powder on the (110) Si at 950 - 1150°C and base pressure 10-4 torr. Some carbon-doped films were also grown and investigated. For optimization of growth conditions the process was carried out under equilibrium and quasi-equilibrium conditions. Obtained under quasi-equilibrium conditions the continuous Mn4Si7 film had a rough surface and a grain structure with an average size of single crystalline grains of a few microns (Figure 1ab). The carbon in the C-doped films formed a nanocrystalline SiC 100÷170 nm-layer that has divided the film into two halves (Figure 1ab). This result differs from another one previously observed for MnSiCx films [2]. The explanation can be first in different growth conditions and second that the X-ray diffraction used in [2] did not possess the capabilities for the local analysis as TEM/EDS. The Mn4Si7 islands on Si substrate were obtained under equilibrium conditions instead of continues film (Figure2a). Sizes of islands are in the range from a few nm to several tens microns. The process of reactive diffusion and formation of Mn4Si7 islands occur in the Si substrate at a depth of a few microns. Electron diffraction analysis showed that micron-size Mn4Si7 islands can contain some cubic MnSi phase inclusions. The sizes of these inclusions could reach 200-250 nm. Figure 2b shows a MnSi inclusion where [112] MnSi // [4 12 5] Mn4Si7. The electrical properties for the films were measured: resistivity and thermoelectric power were about 6⋅10-2 Ω cm and 200-250 μV/K, correspondingly 1. 2. 3.
P. Stadelmann, JEMS. http://cimewww.epfl.ch/. 2008. C. Sürgers, M. Gajdzik, G. Fischer at al. Physical Review B 68 (2003), 174423. We kindly acknowledge the help of CIME-EPFL to use the equipment and software.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 31–32, DOI: 10.1007/978-3-540-85226-1_16, © Springer-Verlag Berlin Heidelberg 2008
32
Figure 1. (a) STEM image of the continues Mn4Si7 film with the SiC layer, EDS linescan is shown for Mn, Si and C elements; (b) TEM and SAED for the single crystalline Mn4Si7 grain and nanocrystalline SiC layer.
Figure 2. (a) TEM image of Mn4Si7 micro- and nanoislands; (b) the inclusion of cubic MnSi in the Mn4Si7 microisland and the corresponding SAED pattern.
33
HR-STEM EELS analysis of silicon 32 nm technology using a TITAN with a probe Cs corrector R. Pantel1, J.L Rouvière2, E. Gautier4, S. Denorme1, C. Fenouiller-Beranger3,1, F. Boeuf1, G. Bidal1 and M. Cheynet5. 1. STMicroelectronics, 850 rue Jean Monnet F-38926 Crolles, France 2. CEA DRFMC 3. CEA LETI 4. CNRS SPINTEC (2, 3, 4) address: MINATEC 17 rue des Martyrs, F-38054 Grenoble, France. 5. SIMaP (UMR 5266) CNRS-INPG-UJF, F-38402 Saint Martin-d’Hères, France
[email protected] Keywords: semiconductor silicon, EELS spectroscopy, HR-STEM, probe Cs corrector.
In this communication we present HRSTEM/EELS studies of 32 nm technology materials and interfaces using a TITAN microscope with a probe Cs corrector. Two examples are presented: silicon direct bounding and metal gates integrating HfZrO2/TiN. It is shown that EELS spectra contain rich material signatures which can help to understand transistor performance variability. The HRSTEM-EELS experiments are carried out at 300 keV using a TITAN with a CEOS probe Cs corrector installed at MINATEC. It is equipped with a Gatan TRIDIEM energy filter and two annular dark field detectors (Gatan ADF and Fischione HAADF). Figure 1a shows a HRSTEM dark field image of a direct silicon bounding (DSB) interface. The purpose of this structure is to provide two crystal orientations in order to improve the carriers mobility for both n and p MOS. The fabrication process uses Si-Si wafer bounding in presence of a thin oxide layer which is removed by high temperature annealing. The STEM Z-contrast image shows an abrupt interface and a dark area 3 nm thick in the top layer. Inside this area no oxygen is detected using EELS analysis, so this dark contrast could be due to vacancies or strain field. Figure 1 b shows a HRSTEM DF image of the bottom of a metal gate integrating Si/SiO2/HfZrO2/TiN. We have observed that on such gates the Vth and the equivalent oxide thickness (EOT) are changing continuously vs the TiN thickness (3 to 15 nm). EELS profiles presented in Figure 2 show that oxygen and nitrogen concentrations in the TiN layer depend on its thickness. In thin TiN layer, the oxygen level is high and the nitrogen low. For thick TiN layers the N/Ti ratio is about one, the oxygen been present only at the upper interface. In order to better understand the material properties low loss EELS profiles where also acquired across two stacks integrating a 12 nm and a 3 nm TiN layers. The recorded (E, x) spectrum profiles are displayed in Figure 3a and 3b respectively (intensity colour scale). These diagrams clearly visualise the different layers through their plasmon signatures. From the EELS line profile series one can extract individual spectrum inside the layers or at the interfaces. Figure 4a and 4b display the low loss spectra recorded in the middle of HfZrO2 (capped with 12 or 3nm TiN) and in the middle of both TiN layers. Significant differences in the low loss signatures are observed, especially in the TiN layers indicating nitrogen depletion in the 3 nm layer whereas a δ-TiN phase is formed in the 12 nm layer. Additional analyses will be carried out to interpret these signatures and S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 33–34, DOI: 10.1007/978-3-540-85226-1_17, © Springer-Verlag Berlin Heidelberg 2008
34
extract electronics properties of the HfZrO2 dielectric layer [1-2]. These results will be presented at the conference including also near edge core loss fine structures analysis. 1. 2.
S. Pokrant, M. Cheynet, S. Jullian and R. Pantel. Ultramicroscopy 104 (2005) 233. M. Cheynet, S. Pokrant, F. Tichelaar and J.L. Rouvière, J. Appl. Phys. 101 (2007), 054101.
Figure 1: STEM Z contrast images, a) DSB silicon interface. b) Si/SiO2/HfZrO2/TiN.
Figure 2: EELS profiles across Si/SiO2/HfZrO2/TiN/Si-poly: (TiN 12, 10, 12, 5, 3 nm).
Figure 3: EELS Low Loss vs scan position across HfZrO2/TiN. a) TiN 12 nm b) 3 nm.
Figure 4: EELS spectra: a) inside HfZrO2, b) in TiN for TiN 3 nm (red) 12 nm (green).
35
Tomographic analysis of a FinFET structure O. Richard, P. Van Marcke and H. Bender IMEC, Kapeldreef 75, B-3001 Leuven, Belgium olivier
[email protected] Keywords: Electron Tomography, Fin Field Effect Transistor
In order to meet the International Technological Roadmap for Semiconductor (ITRS) goals [1] for the 32nm node and beyond new structures as the multiple-gate Silicon on insulator MOSFET (Metal Oxide Semiconductor Field Effect Transistor) with good short channel characteristics and high drive current are introduced [2]. One of the considered configurations is the FinFET (Fin Field Effect Transistor) structure consisting of single crystalline silicon fins with the gate line crossing in the orthogonal direction (Figure 1). Because the typical dimensions of these structures are smaller than the thickness of the TEM specimen, the overlap of different materials along the electron beam direction renders the interpretation of the conventional TEM images (Figure 2) difficult. Tomographic 3D reconstruction from high angular annular dark field scanning (HAADFS) TEM image series can overcome this problem, and is therefore likely the most suited technique in order to characterize such devices. TEM specimens with different geometries, i.e. cylindrical and plane parallel and with the fin parallel and perpendicular to the TEM specimens are prepared by FIB (Focus Ion Beam) milling (FEI, Strata). The acquisition of the HAADF STEM image series is performed with a FEI Tecnai (F30) FEG microscope operating at 300kV using the Explore3D software (FEI). The conventional plane parallel TEM specimens are mounted on the single tilt tomographic holder (Fischione) with the tilt axis parallel to the two perpendicular directions 3 and 1 or 3 and 2 subsequently, whereas the cylindrical specimens are fixed with the cylinder axis parallel to the tilt axis. The alignment of the HAADF STEM images and the 3D reconstruction via two schemes, weighted back projection (WBP) and simultaneous iterative reconstruction (SIRT) with 20 iterations, are performed with the Inspect3D software (FEI). Different slices from the 3D SIRT and WBP reconstructions obtained with the plane parallel sample presented in Figure 2a (tilt axis parallel with the direction 3) and with a cylindrical sample with the fin parallel to the electron beam at 0º (tilt range -70º/+70º, increment step 1º) are presented in Figure 3a-d and in Figure 3e-g, respectively. The HfO2 layer, ~ 2nm thick, exhibiting a bright contrast is detected at the top of the fin and below the polysilicon gate (arrows) and not at the fin sidewalls (Figure 3a), whereas this layer is clearly observed around the fin for the cylindrical sample (Figure 3f). The trapezoidal feature exhibiting a bright contrast on Figure 3b (arrow) comes from the high-k layer, indicating that the HfO2 layer is not properly etched in this area. Such information cannot be obtained from conventional TEM images. The bright contrast observed under the gate in the slice taken in the middle of the fin (arrow) (Figure 3c & 3e) is likely due to an artefact induced by the SIRT reconstruction scheme. This feature
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 35–36, DOI: 10.1007/978-3-540-85226-1_18, © Springer-Verlag Berlin Heidelberg 2008
36
is less observed for the WBP reconstruction (Figure 3d). The nitride spacers (arrows) are clearly observed on the slice presented in Figure 3g. 1. 2. 3.
http://www.itrs.net/ H.-S.P. Wong, IBM J. Res. & Dev. 46 (2002), p. 133. The IMEC Device Implementation Project group is acknowledged for providing the sample.
Figure1. Scheme of a FinFET Figure 2. Cross-section TEM image with the fin structure with indication of the parallel (a) and perpendicular (b) to the TEM axes and plane labelling. specimen. a
b
b
c
c
d
a
e
f
f
g
g
e
Figure 3. Slices from the 3D reconstruction obtained with the fin parallel to the plane parallel specimen and with the tilt axis parallel to the direction 3: Fin in cross-section in the middle of the gate line (a). Slice parallel with the fin length at the level of the fin sidewall (b) and in the middle of the fin width with SIRT (c) and WBP (d) reconstruction scheme. Slices from the 3D reconstruction obtained with a cylindrical sample with the fin parallel to the electron beam at 0º: Slice parallel with the fin length in the middle of the fin width (e). Fin in cross-section in the middle of the gate line (f). Fin in cross-section further away from the gate (g).
37
STEM EELS/EDX dopant analysis of nm-scale Si devices G. Servanton1, R. Pantel1, M. Juhel1 and F. Bertin2 1. STMicroelectronics, 850 rue Jean Monnet, F-38926 Crolles, France 2. CEA-LETI, MINATEC, 17 rue des Martyrs, F-38054 Grenoble, France
[email protected] Keywords: Silicon, Semiconductors, STEM EELS/EDX, Radiation damage, Si As/P doped
The mapping of dopant in Si devices is critical for their performance optimisation. Off-axis electron holography is a TEM based technique that is presently used to provide 2D dopant maps of semiconductor devices [1]. Due to the improvement of electron gun brightness and probe aberration correctors in TEM, the direct detection of dopant atoms is now possible. In this paper we demonstrate dopant profiling using either 200 keV low-dose EELS or 120 keV high-dose EDX. Our results are compared with SIMS. EDX and EELS experiments have been performed in STEM mode with a FEG TECNAI F20 using a EDAX detector and a Gatan Energy filter GIF 200. Samples were prepared and cleaned at low energy (5 keV) with a FEI DB400 FIB. High-energy electrons induce knock-on damage in Si [2], but below a critical energy, the momentum conservation does not allow enough energy transfer and the radiation damages become thus negligible. We evaluate in Figure 1. the critical beam energy for an intense focused probe on Si. The EDX Si signal is monitored to track the etching of the Si during electron beam irradiation. As the specimen is etched, the signal decreases and finally, a hole is observed (see inset in Figure 1.(a)). A 75-nm-thick lamella is completely etched for a (2.5 nA x 20 s) dose at 200 keV; etching also occurs at 160 keV for a dose that is 5 times higher, at 120 keV etching is negligible. This critical energy (120 keV) is lower than the quoted 200 keV [2]. Figure 1.(c) shows the etching probability and Si/Ge EDX signal measured for the same dose using SiGe reference. The 120 keV energy is then ideal for high dose EDX analysis since EDX cross-section of Si (or P) and Ge (or As) are increased. To illustrate EDX analysis versus energy, Figure 2. presents STEM EDX profiles of a P and As doped Si junction at different energy compared to SIMS profile. Each energy gives reasonable results but the dose and signal-to-noise ratio can be increased for an energy below 120 keV. Figure 3. shows the results from a 0.6% As doped Si layer analysed using low dose EELS at 200 keV and high dose EDX at 120 keV. The EELS measurements have high spatial resolution whereas the EDX profile has an excellent signal-to-noise ratio. Figure 4. shows a 120 keV EDX analysis of a BiCMOS transistor. The STEM EDX profile shows As dopant in the emitter (0.3%) and a strong segregation at the epitaxial interface (1%). This process is not optimum for transistor performances. Figure 4. shows a comparison of SIMS (acquired in 300x300 µm² box) with EELS As/Ge profiles in another BiCMOS. EELS and SIMS data are similar both quantitatively and qualitatively. In this case, the process is optimized and EELS allows studying size structure effects on epitaxial growth.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 37–38, DOI: 10.1007/978-3-540-85226-1_19, © Springer-Verlag Berlin Heidelberg 2008
38
In conclusion, the detection of dopant at concentrations 5×1019 cm-3, or below, is possible using EELS/EDX. Other applications will be presented, in particular a study of structure dimension effect during epitaxy and dopant mapping. 1. 2.
W. D. Rau, Phys. Rev. Lett. 82, 2614 - 2617 (1999) D. B. Williams, TEM, A Textbook for Materials Science, Springer (1996), p.63
Figure 1. Visualisation of Si damage using EDX signal with the effect of (a) Si specimen thickness, (b) electron beam energy, and (c) Si etching probability and Si/Ge cross-sections at different beam energies.
Figure 2. P/As junctions analysis with SIMS and EDX profiles for various energies.
Figure 3. (a) EELS (b) EDX profiles, (c) STEM image of a 0.6% As doped Si layer.
Figure 4. (a, c) BiCMOS transistors, (b) EDX, (d) SIMS and (e) EELS As/Ge profiles.
39
Electron beam induced damage: An atom-by-atom investigation with TEAM0.5 C. Kisielowski1, R. Erni1, and J. Meyer2 1. National Center for Electron Microscopy, Lawrence Berkeley National Laboratory, One Cyclotron Rd., Berkeley CA 94720, USA 2. Department of Physics, University of California at Berkeley CA 94720, USA
[email protected] Keywords: InGaN, In2O3, CdS, Ge, C, Aberration-corrected electron microscopy, single atom detection, radiation damage
A next generation electron microscopes is currently being developed by the Department of Energy as a collaborative effort to redesign the instruments around aberration corrected optics [1]. Within this project, the TEAM 0.5 prototype microscope is currently being commissioned. The instrument is equipped with a high brightness gun and a monochromator [2]. However, already in the past concerns were raised [3] and debated [4] that the high current density in field emission microscopes may alter the atomic structure of materials too fast to record undamaged images of compound semiconductors. Concerns about electron beam induced knock-on damage are indeed very relevant because the TEAM project aims at reconstructing the three dimensional structure of materials at atomic resolution, which requires maintaining structural integrity. On the other hand detailed knowledge about knock-on (and ionization) damage in such microscopes is absent and the TEAM0.5 microscope is ideally suited for such investigations since its unprecedented performance allows for the detection of single atoms of most elements of the periodic system. This contribution addresses electron beam induced damage at the single atom level in a variety of materials including InGaN alloys, In2O3, CdS, Ge and graphene. Two examples are shown in Figures 1 and 2. We find that previous investigations of beam induced atom and atom column displacements at the gold vacuum interface [5] are also observed in seminconductors and that electron beam damage scales with the strength the atoms are bound to their neighbours. Therefore, surface or edges atoms are affected most and the electron beam commonly stimulates surface diffusion. However, even if extreme illumination conditions are employed as reported in Figures 1 and 2 we find that beam induced damage is controllable at the single atom level and that even the amorphous structure of weakly bound adsorbates can be resolved in single images if 80kV of acceleration voltage is utilized. [6] 1. 2.
http://ncem.lbl.gov/TEAM-project/index html C. Kisielowski, B. Freitag, M. Bischoff, H. van Lin, S. Lazar, G. Knippels, P. Tiemeijer, M. van der Stam, S. von Harrach, M. Stekelenburg, M. Haider, S. Uhlemann, H. Müller, P. Hartel, B. Kabius, D. Miller, I. Petrov, E. A. Olson, T. Donchev, E.A. Kenik, A. Lupini, J. Bentley, S. Pennycook, I.M. Anderson, A.M. Minor, A.K. Schmid, T. Duden, V.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 39–40, DOI: 10.1007/978-3-540-85226-1_20, © Springer-Verlag Berlin Heidelberg 2008
40
3. 4. 5. 6.
Radmilovic, Q. Ramasse, M. Watanabe, R. Erni, E.A. Stach, P. Denes, U. Dahmen, submitted (2008). M. Galtrey, R. Oliver, M. Kappers, C. Humphreys, D. Stokes, P. Clifton, and A. Cerezo, Applied Physics Letters 90 (6), 061903 (2007). C. Kisielowski and T. Bartel, Applied Physics Letters (2007). V.A. Martin, K. Ishizuka, C. Kisielowski, and L.J Allen, Phys. Rev. B 74, 172102 (2006). The TEAM project is supported by the Department of Energy, Office of Science, Basic Energy Sciences. NCEM is supported under Contract # DE-AC02-05CH11231.
Figure 1. Reconstructed phase images of In2O3 [011] from a focal series of 26 lattice images. a) Phase from images 1-13 with model inserted b) Phase from images 14-26. The crystal is oxygen terminated. The arrow marks an atom column that disappears after recording image 13. Reconstruction aperture: 0.5 Å; 300 kV; recording interval between images: 3 sec; current density: 3 104 e/Å2s; monochromator switched on.
Figure 2. a) Lattice image of graphene with monolayer adsorbates. Carbon atoms are imaged bright. b) The lattice fringes of the monolayer graphene sheet are removed from the image. The amorphous structure of the adsorbate is resolved in single images. 80 kV; current density: 1.4 105 e/Å2s; monochromator switched on.
41
The atomic structure of GaN-based quantum wells and interfaces C.J. Humphreys1, M.J. Galtrey1, R.A. Oliver1, M.J. Kappers1, D. Zhu1, C. McAleese1, N.K. van der Laak1, D.M. Graham2, P. Dawson2, A Cerezo3 and P.H. Clifton4. 1. Department of Materials Science and Metallurgy, University of Cambridge, Pembroke Street, Cambridge CB2 3QZ, UK. 2. School of Physics and Astronomy, Alan Turing Building, University of Manchester, Manchester M13 9PL, UK 3. Department of Materials, University of Oxford, Parks Road, Oxford OX1 3PH, UK 4. Imago Scientific Instruments, 5500 Nobel Drive, Madison, Wisconsin 53711, USA
[email protected] Keywords: gallium nitride, quantum wells, interfaces
We have used a combination of high resolution electron microscopy (HREM), three dimensional atom probe (3DAP) microscopy and atomic force microscopy (AFM) to reveal the atomic structure of InGaN quantum wells (QWs) and InGaN interfaces. Such quantum wells and interfaces are of considerable scientific and technological importance because they form the basis of GaN-based LEDs and lasers. A long-standing puzzle has been why GaN-based LEDs emit brilliant light when the dislocation density is so high. Originally it was believed that this was because the excitons (bound electron-hole pairs which recombine, emitting light) were localized in indium-rich clusters in the InGaN quantum wells and so could not diffuse to dislocations, which would quench the light emission. However, careful HREM work showed this was not the case [1], and this was confirmed by 3DAP images that showed that InGaN was a random alloy, up to at least 25% In content [2]. If there are no In-rich clusters in the InGaN QWs, what mechanism is responsible for localizing the excitons and preventing them from diffusing to dislocations? HREM images suggest that the lower GaN/InGaN QW interface is flat and the upper InGaN/GaN QW interface has monolayer steps several nm across [3]. 3DAP images strikingly confirm this, see Figure 1 [4]. Because of the strain in the QW and the strong piezoelectric effect in InGaN, a monolayer interfacial step is sufficient to localize the carriers at room temperature and prevent them from diffusing to dislocations [3]. If an InGaN QW is grown at the same temperature as the GaN barriers, a uniform QW results (with interface steps on its upper surface). However, two-temperature growth is commonly used, in which the GaN barriers are grown at a higher temperature than the InGaN QW. In this case HREM, AFM and 3DAP reveal that the quantum well can break-up into a network structure, on a 50-100nm lateral length scale. The threading dislocations mostly pass through the gaps in the QWs, and this provides an additional localization mechanism, on a longer length scale, see Figure 2 [5,6]. 3DAP reveals that a low level of In is present in the GaN barriers although the In flux is switched off during growth of the barriers, and this occurs for both blue and
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 41–42, DOI: 10.1007/978-3-540-85226-1_21, © Springer-Verlag Berlin Heidelberg 2008
42
green emitting QW structures. The source of this In appears to be the InGaN QW layers, with In segregating, not diffusing, into the barriers from the QWs [4]. We conclude that HREM, 3DAP and AFM form a powerful combination of microscopy techniques for studying the atomic structure of quantum wells and interfaces in semiconductors. 1. 2. 3. 4. 5. 6.
T. M. Smeeton, M. J. Kappers, J. S. Barnard, M. E. Vickers and C. J. Humphreys, Appl. Phys. Lett. 83 (2003), 5419. M. J. Galtrey, R. A. Oliver, M. J. Kappers, C. J. Humphreys, D. J. Stokes, P. H. Clifton and A. Cerezo, Appl. Phys. Lett. 90 (2007), 061903. D. M. Graham, A. Soltani-Vala, P. Dawson, M. J. Godfrey, T. M. Smeeton, J. S. Barnard, M. J. Kappers, C. J. Humphreys and E. J. Thrush, J. Appl. Phys. 97 (2005), 103508. M. J. Galtrey, R. A. Oliver, M. J. Kappers, C. J. Humphreys, P. H. Clifton, D. Larson, D. W. Saxey and A. Cerezo, J. Appl. Phys. (2008), submitted. N. K. van der Laak, R. A. Oliver, M. J. Kappers and C. J. Humphreys, Appl. Phys. Lett. 90 (2007), 121911. M. J. Galtrey, R. A. Oliver, M. J. Kappers, C. McAleese, D. Zhu, C. J. Humphreys, P. H. Clifton, D. Larson and A. Cerezo, Appl. Phys. Lett. 92 (2008), 041904.
Figure 1. 3D atom probe image of the (a) upper and (b) lower interfaces of an InGaN/GaN quantum well emitting in the green (25% In content in the well), showing interface steps on the upper interface.
50 nm
Figure 2. Cross-sectional STEM-HAADF image of a commercial bright green LED showing gross thickness variations (arrowed) in all four InGaN quantum wells.
43
Using TEM to investigate antiphase disorder in GaP films grown on Si(001) T.B. Adams1, I. Nemeth1, G. Lukin1, B. Kunert2, W. Stolz1, K. Volz1 1. Materials Science Centre, Philipps-University Marburg, D-35032, Germany 2. NAsP III/V GmbH, D-35041, Germany
[email protected] Keywords: dilute nitride; defects; MOVPE
GaP-based dilute nitride materials are of great technological interest since Ga(NAsP) exhibits a direct band-gap and can be grown pseudomorphically-strained on Si substrates. Multi-quantum-well laser devices grown on GaP substrates have already been demonstrated with efficient and stable performance[1], and the growth of such devices on nominally exact Si(001) would represent a tremendous technological leap forward, allowing the incorporation of optoelectronic devices into silicon chips by conventional CMOS fabrication. To date, however, completely defect-free dilute nitride films grown directly on Si(001) have not been achieved. Since Ga(NAsP) can be grown defect-free on GaP, and GaP can in principle be grown on Si(001), one possible solution is to use GaP as a buffer layer between the Si substrate and Ga(NAsP) layer(s). Growth of defect-free GaP on Si presents its own challenges: conditions must be such that planar defects such as twins and stacking faults are eliminated. Anti-phase domain boundaries (APB) represent a special case of planar defect, where the polarity of the crystal is inverted on either side of the domain. Polarity inversion can be regarded as a 90o rotation of the crystal about the axis perpendicular to the plane of the substrate/film interface. APB’s originate from inhomogenous nucleation of the 1st monolayer of GaP, from mono-steps on the Si surface, or from a thermodynamic need to distribute interfacial charge at the GaP/Si interface. The density of APB nucleation sites on exact-oriented Si substrates can be minimised by appropriate substrate preparation and the remaining APB’s can, under certain growth conditions, ‘kink’ so that they connect and self-annihilate before reaching the GaP surface. APB’s can therefore be tolerated in the GaP buffer layer, provided they have self-annihilated before reaching the buffer layer surface. The TEM is an indispensable tool for characterising APB morphology and for providing critical information to allow optimisation of growth conditions. APB’s can be imaged directly using HR-TEM and dark field imaging (see Figure 1, for example), while the polarity can be determined locally using convergent beam electron diffraction. The application of these techniques in the growth of GaP on Si(001) by Metal Organic Vapour Phase Epitaxy will be discussed and defect structure will be correlated to growth conditions. 1.
B. Kunert, A. Klehr, S. Rheinhard, K. Volz, W. Stolz, Electronics Letters 42 (2006)
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 43–44, DOI: 10.1007/978-3-540-85226-1_22, © Springer-Verlag Berlin Heidelberg 2008
44
Figure 1. Dark field image pair showing morphology of antiphase domains in a GaP buffer layer grown in Si(001).
45
TEM characterization of InAs/GaAs quantum dots capped by a GaSb/GaAs layer A.M. Beltrán1, T. Ben1, A.M. Sánchez1, D.L. Sales1, M.F. Chisholm2, M. Varela2, S.J. Pennycook2, P.L. Galindo3, J.M. Ripalda4 and S.I. Molina1 1. Dep. Ciencia de los Materiales e Ing. Met. y Qca. Inorg., Facultad de Ciencias, Universidad de Cádiz. Campus Río San Pedro, Puerto Real 11510 Cádiz, Spain 2. Materials Science and Technology Division, Oak Ridge National Laboratory, 37831 Oak Ridge, Tennessee, USA 3. Dep. Lenguaje y Sistemas informáticos, CASEM, Universidad de Cádiz, Campus Río San Pedro, Puerto Real 11510 Cádiz, Spain 4. Instituto de Microelectrónica de Madrid (CNM-CSIC) Isaac Newton 8, 28760 Tres Cantos, Madrid, Spain
[email protected] Keywords: InAs QDs, TEM, GaSb
It is well known that there is intense interest in expanding the usable wavelength for electronic devices. Research efforts are dedicated to develop GaAs technology in order to achieve emission at 1.3 and 1.55 µm, so GaAs could be used for telecommunication applications [1]. Ga(As)Sb on InAs/GaAs quantum dots (QDs) is a promising nanostructure to be used in telecommunications. The introduction of antimony to these nanostructures is an effective solution to obtain redshift emission, even at room temperature [2]. Several authors have reported a miscibility gap for GaSb and InAs in absence of strain [3]. Our preliminary studies by Conventional Transmission Electron Microscopy (CTEM) of nanostructures on GaAs (001) substrates show the formation of a quaternary alloy InxGa1-xAsySb1-y when a GaSb layer is grown over the QDs. In order to achieve a proper formation of the system InAs QDs/GaSb barrier layer, the growth of an intermediate GaAs layer between the InAs QDs and the GaSb cap layer resulted as a promising growth solution. In this work we have studied the effect of the introduction of intermediate layers with diverse thickness comparing with InAs QDs directly capped. Studied samples have been grown by molecular beam epitaxy on GaAs (001) substrate. InAs was deposited, followed by a GaSb or GaAs/GaSb layers. Finally, the nanostructure was capped by GaAs [4]. In this work we have analysed sample A (without GaAs intermediate layer), sample B1, B2 and B3 with 3, 6 and 12 MLs of GaAs intermediate layer respectively. The structural characterisation of these samples was carried out by TEM in a JEOL 1200EX and 2011EX at 120 and 200 kV respectively. During this study dark field (DF) g002 cross-section (XTEM) images were taken from samples A, B1 and B2 (see Figure 1a for sample A). These images show in general dots with a brighter core than the GaAs substrate which are formed on and surrounded by GaAs. In these images the GaSb layer can not be clearly distinguished. In accordance with g002DF intensities dynamically simulated by EMS software (not shown in this work), GaSb layers have brighter
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 45–46, DOI: 10.1007/978-3-540-85226-1_23, © Springer-Verlag Berlin Heidelberg 2008
46
contrast than GaAs and InAs layers for sample thickness lower than 50 nm (case conscientious chosen for this study). In view of these results a GaSb layer mixed with GaAs, and maybe with InAs (from QDs and intermediate layers), seems to have been formed. However, on sample B3 (see Figure 1b) a layer with brighter contrast than GaAs substrate can be undoubtedly observed on the intermediate layer, which can be related to a GaSb layer. It could be said that depositing 12 MLs of GaAs avoids the intermixing of GaSb with GaAs intermediate layer and, therefore, with InAs. In order to clarify the type of InGaAsSb alloy inside dots, compositional studies initially on sample A were carried out by high resolution scanning transmission electron microscopy (STEM) using a high-angle annular dark field (HAADF) detector and spatially resolved electron energy loss spectroscopy (EELS) in two dedicated scanning transmission microscopes. Taking GaAs as reference for Ga and As, In and Sb maps were calculated as 100-CGa and 100-CAs, respectively (CGa and CAs represent Ga and As concentration) from low loss EEL spectra. These studies have demonstrated the presence of the four elements inside the QDs in an estimated concentration of 40% (~20% at the wetting layer). These results have been confirmed by the analysis of HAADF images. Since in this technique higher intensity is associated with higher atomic numbers (Z), the position of the maximum of an intensity profile would correspond with the area of the highest concentration of In/Sb. The maximum is located in the central region of the QD which is associated with the quaternary alloy InxGa1xAsySb1-y [5]. In conclusion, it has been shown that the presence of a GaAs intermediate layer between the InAs QDs and the GaSb layer improves structural quality and minimise the intermixing of the binary compound semiconductor constituting the nanostructure, as the GaAs thickness increases over 6 MLs. Compositional analyses have demonstrated the formation of a quaternary alloy inside the QDs when GaSb is grown over InAs QDs. 1. V.M. Ustinov and A.E. Zhukov, Semicond. Sci. Technol. 15 (2000) p. R41. 2. J. M. Ripalda, D. Granados, Y. González, A.M. Sánchez, S.I. Molina and J.M. García, Appl. 3. 4. 5. 6.
Phys. Lett. 87 (2005) 202108. G.B. Stringfellow, J. Cryst. Growth 58 (1982) p. 194. J. M. Ripalda, D. Alonso-Álvarez, B. Alén, A. G. Taboada, J. M. García, Y. González and L. González, Appl. Phys. Lett. 91 (2007) 012111. S.I. Molina, A.M Sánchez, A.M Beltrán, D.L Sales, T. Ben, M.F. Chisholm, M. Varela, S.J Pennycook , P.L. Galindo, A.J. Papworth, P.J. Goodhew and J.M Ripalda, Appl. Phys. Lett. 91 (2007) 263105. This work has been supported by MEC (TEC2005-05781-C03-01 and 02/MIC), SANDiE European network (Contract NMP4-CT-2004-500101), Junta de Andalucía (PAI research group TEP-120) and U.S. Department of Energy, Division of Materials Science and Engineering (MFC, MV and SJP). We acknowledge Prof. P. J. Goodhew and Dr. A. J. Papworth for the use of the STEM facilities in the University of Liverpool. a)
QDs
GaAs substrate
GaAs cap layer
25 nm
b) GaAs substrate
GaAs cap layer QD
GaSb
Figure 1. XTEM DF g002 images of samples a) A and b) B3.
25 nm
47
The microstructure of (0001)GaN films grown by molecular beam epitaxy from a nanocolumn precursor layer D. Cherns1, L. Meshi1, I. Griffiths1, S. Khongphetsak1, S.V. Novikov2, N. Farley2, R.P. Campion2, and C.T. Foxon2 1. Department of Physics, University of Bristol, Tyndall Avenue, Bristol, UK 2. Department of Physics and Astronomy, University of Nottingham, Nottingham, UK
[email protected] Keywords: GaN, polarity, crystal growth, dislocation reduction
A major challenge in the production of GaN devices is to reduce the densities of threading dislocations, typically up to 109 – 1011 cm-2, generated by the use of highly mismatched substrates such as (0001)sapphire. One method is to use epitaxial lateral overgrowth (ELO) where a mask is used to restrict the growth of the GaN to “seed” columns. Lateral growth leads to “wings” where dislocation densities may be several orders of magnitude less than in the seed. In this paper we consider a maskless ELO approach in which the GaN is grown on (0001)sapphire. Firstly, GaN is grown by molecular beam epitaxy under strongly N-rich conditions, leading to pronounced nanocolumn growth [1]. The growth is then continued under Ga-rich conditions, leading to lateral growth and coalescence of the nanocolumns. Eventually, continuous GaN layers are formed with threading dislocation densities in the range 108 – 109 cm-2. Growth was carried out using plasma-assisted MBE (PA-MBE) in a Varian ModGen II MBE system. A 5nm AlN buffer layer was grown at a temperature of 600°C prior to the GaN growth at 700-800°C. Following up to 6 hours of growth in a high overpressure of active nitrogen provided by an HD25 RF activated plasma source, the N flow was reduced and growth continued for 1-6 hours under Ga-rich conditions. TEM samples were prepared in cross-sectional orientation, either by mechanical polishing followed by Ar-ion thinning in a Gatan PIPS, or by sectioning in an FEI 201 focused ion beam thinner (FIB), and examined at 200kV in a JEOL 2010 TEM. SEM studies were also carried out on as-grown samples using a JEOL JSM7400F FEGSEM. Figure 1 shows a sample grown only under N-rich conditions. This contains a rough, but mostly continuous, intermediate GaN layer extending up to 400 nm from the substrate. In addition, there are discrete GaN nanocolumns which protrude through this layer up to around 2 μm from the substrate. Close inspection indicates that the nanocolumns contain relatively few defects, with contrast mainly consisting of bend contours. In contrast, the intermediate layer is highly defective, containing both threading dislocations and high densities of basal plane stacking faults, which are near edge-on and mostly out of contrast in this figure. The polarity of the deposit was examined by taking convergent beam electron diffraction (CBED) patterns under symmetrical (0002) systematic row conditions, i.e. with ±0002 reflections at the same deviation parameter. Under these conditions, the intensities in ±0002 reflections differ owing to double
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 47–48, DOI: 10.1007/978-3-540-85226-1_24, © Springer-Verlag Berlin Heidelberg 2008
48
diffraction contributions [2]. The nanocolumns were found to be Ga-polar, and the intermediate layer N-polar. Figure 3 illustrates a layer grown firstly under N-rich conditions and then under Garich conditions. The nanocolumns have grown laterally near the column tops, leading to a continuous overlayer. Coalescence of the nanocolumns gives appreciable areas which are free of threading defects, but with occasional threading defects describing the coalescence of nanocolumns which are locally misoriented. In contrast, the N-polar underlayer has undergone negligible further growth under Ga-rich conditions. Figure 3 demonstrates that nanocolumn growth provides a successful method of reducing threading dislocation densities in GaN films. In the paper, the mechanisms of nanocolumn growth and of dislocation reduction will be illustrated and explained. 1. 2. 3.
E. Calleja et al , Phys. Stat. Sol. b 244, 2816-2837 (2007) D. Cherns et al, Phil. Mag.A77 273-286 (1998) This work was supported under an EPSRC grant EP/D080762/1
Figure 1. SEM (left) and TEM (right) showing Ga-polar nanocolumns protruding from an intermediate layer of N-polar GaN, grown for 6 hrs by MBE under N-rich conditions.
Figure 2. GaN layer grown for 5 hrs under N-rich conditions and then 5 hrs under Garich conditions showing a continuous Ga-polar overlayer (growth surface: bottom right).
49
Compositional and Morphological Variation in GaN/AlN/AlGaN Heterostructures P.D. Cherns, C. McAleese, M.J. Kappers and C.J. Humphreys Department of Materials Science and Metallurgy, University of Cambridge, Pembroke St, Cambridge, CB2 3QZ, UK peter.cherns@cea fr Keywords: AlGaN, STEM, EFTEM
AlGaN/GaN heterostructures are an important materials system for the development of optoelectronic devices emitting in the ultraviolet region of the electromagnetic spectrum. Due to a difference in lattice parameter between GaN (a=0.31893 nm) and AlN (a=0.31130 nm), AlGaN grows under tensile strain on GaN. This leads to cracking above a critical thickness, which decreases with increasing Al content. It has been shown that this problem can be overcome by the use of low [1] or high [2] temperature-grown AlN interlayers. The function of the interlayer is to relax sufficiently without macroscopic cracking, in order to exert compressive strain on the subsequently grown AlGaN layers. In this paper, we present a study of AlN interlayers by high-angle annular dark field (HAADF) imaging and energy-filtered transmission electron microscopy (EFTEM). The work focuses on the morphological and compositional variations that result from changes in growth temperature and growth time. The samples are grown on c-plane sapphire by metal organic vapour phase epitaxy (MOVPE). Interlayer growth temperatures were varied between 700°C and 1020°C, and thicknesses between 1 nm and 50 nm. It is shown that the use of AlN interlayers thicker than 5 nm is effective in preventing cracking in AlGaN layers, which is independent of growth temperature. However, it has been seen that changes in growth temperature do have a significant impact on the composition and morphology of the interlayers. High resolution HAADF images of 5 nm and 10 nm interlayers grown at 1020°C are presented in Figure 1. The images show examples of frequently observed trench-like features in the interlayers, as well as an indication of changes in interlayer composition. To study composition changes at high and low growth temperature, EFTEM filtered series were acquired around the Ga L2,3 edge at 1115 eV. A 20 eV energy selecting slit was used and 18 images were acquired at 20 eV spacing. The resultant Ga maps, as presented in Figure 2, shows that at higher growth temperatures the Al content is inhomogeneous in the interlayers. Ga is present in the interlayer in contrast to the pure AlN that is expected. There is vertical segregation of material, with Al-rich material near the top of the layer. The trenches are observed more frequently as the growth temperature is increased and experimental evidence indicates that Al is favourably incorporated around the edges of the features. Possible mechanisms for the formation of these trenches are discussed.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 49–50, DOI: 10.1007/978-3-540-85226-1_25, © Springer-Verlag Berlin Heidelberg 2008
50
This study has important implications for the understanding of the growth of AlGaN/GaN heterostructures, particularly in relation to the incorporation of Al under tensile strain. 1. 2.
H. Amano, M. Iwaya, N. Hayashi, T. Kashima, S. Nitta, C. Wetzel and I. Akasaki, Physica Status Solidi (b) 216 (1999), p683. I.H. Lee, T.G. Kim and Y.Park, Journal of Crystal Growth 234 (2002), p305.
Figure 1. HR-HAADF images from samples with (a) 5 nm and (b) 10 nm AlN interlayers, grown at 1020°C. Images are acquired with sample oriented along a <1120> zone axis.
Figure 2. (a) EFTEM Ga maps, presented both raw and corrected for thickness variation and elastic scattering, taken from samples with 30 nm AlN interlayers grown at 700°C and 1020°C. (b) Intensity profiles taken from the two corrected Ga maps, normalised to 100% Ga content in the GaN template.
51
TEM/STEM/EFTEM imaging and Valence Electrons Spectroscopy analysis of Ultra Low-K dielectrics M. Cheynet1, S. Pokrant2, M. Aimadeddine3, V. Arnal3, F. Volpi1 1. Laboratoire SIMaP 1130 rue de la Piscine BP75 Saint Martin d’Hères 38042 France 2 Carl Zeiss NTS GmbH, 73447 Oberkochen, Deutschland. 3. ST Microelectronics Rue Jean Monnet, 38920 Crolles, France
[email protected] Keywords: Ultra-Low-k, electronic properties, TEM-STEM imaging, EFTEM, VEELS.
The ITRS requires the integration of dielectric materials with effective dielectric constant (k) lower than 2.8 [1]. This is achieved using porous organic silicate glass in full-sheet deposition. Unfortunately, during the integration processes several steps like lines etch or Cu Chemical Mechanical Polishing (CMP) introduce damages [1]. One issue, to avoid this damage, is the deposition of a SiO2 based capping layer before the CMP. In this work, we report on the results deduced from imaging techniques performed in the environment of TEM (i.e. BF/DF TEM and STEM imaging, EFTEM and Z-contrast imaging), and on the results deduced from Valence Electron Energy Loss Spectroscopy (VEELS) analysis, both performed to quantify the capping layer effect on the density, the chemistry and the dielectric properties of the low-k layer. 1 – Microstructure and density of “capped” and direct CMP low-k layers: STEM bright/dark field and EFTEM images are recorded from 100 nm thick fibbed TEM foils of “capped” and “direct” CMP low-k samples. For “direct” CMP samples, severe damages are revealed within the Low-K layer. These damages are observed at depth of several tens of nanometers from the polishing surface. They mainly correspond to a decrease of the Low-K material density as indicated by the zero and plasmon loss profiles recorded across the Low-K layers. On the contrary, for “capped” samples, homogeneous contrast and profile are observed in the whole Low-K layer thickness, indicating that, neither significant physical damages nor chemical changes occur. No severe chemical damage is observed, except a small carbon depleted layer wrapping the Cu interconnects lines as shown in the EFTEM images displayed in Figure 2. 2 – Band gap mapping across the “capped” and “direct” CMP ULK layers. SiOCH based low-k samples are transparent to electron for a thickness higher than 200 nm. This allows using thicker TEM foils than usually for low-loss analysis and excludes surface excitation modes to be detected in the low-loss spectra. Moreover, since the refractive index of conventional Low-K materials are reported to be lower than 1.4, Cerenkov losses can be also excluded even working at 200 kV acceleration voltage. The signatures observed in the single scattering low-loss spectra (SSD) can be thus all attributed to electronic transitions after the removal of the zero-loss peak and of the plural scattering from the experimental spectrum. Similar SSD are obtained independently of ZL peak deconvolution procedure applied (Pearson VII function, Richardson Lucy deconvolution [2]). Figure 3 illustrates the band gap determination for
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 51–52, DOI: 10.1007/978-3-540-85226-1_26, © Springer-Verlag Berlin Heidelberg 2008
52
the CMP capped sample. Figure 4 illustrated the result of the band gap and defects energy mapping across the capped and direct CMP Low-K layers. The nanometer scale low-loss maps show that the band gap profile within the capped ULK layer is flat, while it is deeply disturbed in the “direct CMP” layer. The CMP process generates defects close to the conduction band, which is detrimental for the electrical behaviour of the integrated ULK layers. The protection role of the SiO2 based capping layer is clearly demonstrated. 1. K. Maex, M. R. Baklanov, D. Shamiryan, F. Lacopi, S.H. Brongersma and Z. S. Yanovitskaya, J. Appl. Phys. 93, 8793 (2003).
2.
Acknowledgement to Jaysen Nelayah from the LPS d’Orsay in France for the treatment of the low-loss spectra using a Richardson-Lucy deconvolution
Figure 1: TEM cross-section image of the 5th ML of the studied stack, for the capped (left) and the direct CMP (right) samples. Zero-loss and low-loss profiles recorded in the Low-K layer showing strong density variations in the direct CMP sample. Figure 2: C-K edge, O-K edge, C-K/O-K edges EFTEM images showing a carbon depleted layer wrapping the Cu lines
Figure 3. Band gap and defects energy transition determination for “capped” low-k layer.
Figure 4. Band gap and defect energy signature profiles along the ULK layer of the “direct CMP” sample (left) and the “capped” sample (right) showing the protection role of the SiO2 based capping layer
53
Epitaxial Orientations of GaN Grown on R-plane Sapphire J. Smalc-Koziorowska1,3, G.P. Dimitrakopulos1, Ph. Komninou1, Th. Kehagias1, S.-L. Sahonta1, G. Tsiakatouras2 and A. Georgakilas2 1. Department of Physics, Aristotle University of Thessaloniki, GR 54124 Thessaloniki, Greece 2. Microelectronics Research Group, Department of Physics, University of Crete, P.O. Box 2208, 71003 Heraklion-Crete, Greece, and IESL, FORTH, P.O. Box 1527, GR 71110 Heraklion-Crete, Greece 3. Department of Materials Science, Warsaw University of Technology, 02-507 Warsaw, Poland
[email protected] Keywords: nonpolar Gallium Nitride, Transmission Electron Microscopy, epitaxy
Nitride-based heterostructure nanostructures grown along non-polar plane orientations are recently investigated for optoelectronic device applications. Such orientations are promising in order to eliminate the high interface charge densities and spatial separation of carrier wave functions in quantum well structures, which are due to the built-in polarization along the [0001] direction of the wurtzite structure. One possible substrate for growth of a-plane ( 1 1 20 ) III-nitrides is r-plane ( 1 1 02 ) sapphire, and growth of both GaN and AlN epilayers on such substrates by various epitaxial techniques has already been reported. In this work the studied gallium nitride films were grown by nitrogen radio-frequency plasma source molecular beam epitaxy (RFMBE) on nitridated r-plane sapphire substrates. Transmission electron microscope (TEM) investigation has shown the presence of misoriented gallium nitride islands at the epilayer/substrate interface, with average diameter ~10 nm “Figure 1”. The misoriented crystallites were overgrown by the nonpolar a-plane GaN, and they were promoted by the presence of interfacial steps on the sapphire surface, introduced by the nitridation. The matrix aplane GaN exhibited the [ 1 100 ]GaN//[ 1 1 20 ]sapphire [0001]GaN//[ 1 101 ]sapphire epitaxial relationship, whereas the orientation relationship of the misoriented islands was [ 01 1 0 ]GaN//[ 1 101 ]sapphire , (0001)GaN~//( 2 1 1 3 )sapphire “Figure 2(a)”, i.e. the islands were semipolar. It was determined that the islands nucleated directly on the sapphire surface and in particular on { 2 1 1 3 } step risers. Furthermore, pockets of sphalerite structure were introduced at low growth temperature as a result of the superposition of basal-plane stacking faults along the [0001] growth direction inside these grains “Figure 2(b)”. Crystallographically equivalent variants of the secondary orientation led to the introduction of twinning “Figure 2(a)”. These phenomena were usually confined close to the epilayer/substrate interface, although some larger misoriented islands reaching the epilayer surface were also observed. [1] 1.
Work supported under the European Community's Marie Curie Research Training Network PARSEM (MRTN-CT-2004-005583)
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 53–54, DOI: 10.1007/978-3-540-85226-1_27, © Springer-Verlag Berlin Heidelberg 2008
54
Figure 1. Cross-section xTEM bright-field image taken under two-beam conditions off the [ 1 100 ]GaN zone axis with gGaN = 0002. The sapphire substrate is out of contrast. Areas of moiré fringes indicate the presence of misoriented islands.
(a)
(b)
Figure 2. (a) Selected area electron diffraction pattern including the sapphire substrate (black solid line, [ 1 101 ]sapph za), nonpolar a-plane GaN (white solid line, [0001] za) and two variants of semipolar GaN (black and white dashed lines, < 01 1 0 >GaN za). (b) Cross-section HRTEM image of the interfacial area between GaN epilayer and sapphire substrate viewed along the [ 1 011 ]sapphire direction inclined at ~77o relative to the substrate normal.
55
Microstructure and growth model of MBE-grown InAlN thin films S.-L. Sahonta1, A. Adikimenakis2, G.P. Dimitrakopulos 1, Ph. Komninou1, H. Kirmse3, E. Pavlidou1, E. Iliopoulos2, A. Georgakilas2, W. Neumann3 and Th. Karakostas1 1. Solid State Physics Section, Department of Physics, Aristotle University of Thessaloniki, 54124 Thessaloniki, Greece 2. Microelectronics Research Group, IESL, FORTH, PO Box 1527, 71110 Heraklion, Crete, Greece and Department of Physics, University of Crete, PO Box 2208, 71003 Heraklion, Crete, Greece 3. Institut für Physik, Humboldt-Universität zu Berlin, AG Kristallographie, Newtonstrasse 15, D-12489 Berlin, Germany
[email protected] Keywords: indium, nitrides, GaN, MBE, HEMT
III-nitride materials are used in a variety of optoelectronic devices due to their high carrier mobility and high current densities. Recently optoelectronic waveguides and field effect transistor junctions are being fabricated with a new type of heterostructure based on In0 18Al0 82N/GaN, as this provides a large band gap difference at the heterojunction coupled with lattice-matching to GaN, inhibiting the formation of straininduced defects known to reduce carrier recombination and mobility [1]. Despite its attractive properties, InAlN growth is challenging owing to the very different optimum growth temperatures for InN and AlN films, requiring InAlN to be grown at a temperature low enough to prevent dissociation of InN, yet high enough to allow sufficient aluminium adatom surface diffusion to deposit high crystalline quality film. There are to date very few studies on the microstructure and morphology of InAlN films, yet such observations are vital in order to fabricate InAlN-based devices with the greatest performance, and to understand the basic structural properties of InAlN. In this work transmission electron microscopy (TEM) is used to characterise a variety of high quality InAlN films grown by molecular beam epitaxy (MBE) on AlN/sapphire (0001) and GaN/sapphire (0001) substrates. Indium alloy contents are varied to allow different conditions of epitaxial lattice mismatch. For all mismatch conditions studied it is found that the InAlN films are deposited as hexagonal columnar grains with distinct {11-20}- and {1-100}-faceted grain boundaries, often lined with threading dislocations. A corresponding transition from 2D to 3D growth mode is observed by reflection high energy electron diffraction (RHEED) during the deposition of the first few nanometres of film, indicating island coalescence. Crystallite grain size is on average 15 nm in diameter regardless of InAlN interfacial lattice mismatch, with slight lateral misalignment of adjacent crystals, resulting in a rough stepped film surface, confirmed by atomic force microscopy (AFM). TEM mass contrast and highangle annular dark field (HAADF) studies (Figure 1) show indium accumulation at the grain boundaries in between the columns. Energy-dispersive X-ray spectroscopy
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 55–56, DOI: 10.1007/978-3-540-85226-1_28, © Springer-Verlag Berlin Heidelberg 2008
56
(EDXS) shows an In content of 51 ± 2 atomic % at the grain boundaries. Eventual film planarisation and compositional homogeneity does not occur after prolonged growth, with the In-rich grain boundaries continuing to the film surface even in thick films (Figure 2). A new growth model is proposed in which the observed non-uniform indium distribution is attributed to film deposition kinetics. 1.
J. Xie, X. Ni, M. Wu, J.H. Leach, Ü. Özgür and H. Morkoç, Applied Physics Letters 91 (2007), p. 132116.
2.
Support by the European Community's Marie Curie Research Training Network PARSEM (MRTN-CT-2004-005583) is gratefully acknowledged.
(a)
(c)
(b)
10 nm
10 nm
10 nm
Figure 1 (a). [0001] TEM image of In0 19Al0 81N film on GaN. Grains of around 15 nm diameter have facets aligned with {1-100} and {11-20}. Pronounced dark mass contrast at grain boundaries indicates accumulation of heavy In atoms; bright mass contrast InAlN shows high Al content in grain centres. (b) [0001] TEM image of In0 12Al0 88N film on AlN shows the same structure as (a). (c) HAADF image of the same film as (b), heavy In atoms appear with bright AlN contrast, confirming segregation of In to the grain edges. Figure 2. Cross sectional bright-field TEM image of a thick In0 12Al0 88N film on GaN, taken with g = 0002, showing periodic vertical contrast due to threading dislocations and scattering from vertical grain boundaries.
100 nm
2
57
Silicon carbide modulated structures as a result of the introduction of 8H bands in a 4H matrix N. Frangis1, M. Marinova1, I. Tsiaoussis1, E.K. Polychroniadis1, T. Robert2, S. Juillaguet2, J. Camassel2 1. Solid State Physics Section, Department of Physics, Aristotle University of Thessaloniki, GR-54124 Thessaloniki, Greece 2. Groupe d'Etude des Semiconducteurs, CNRS and Université Montpellier 2, cc 074-GES, 34095 Montpellier cedex 5, France
[email protected] Keywords: silicon carbide, high-resolution electron microscopy, modulated structures
Due to its excellent physical properties, silicon carbide (SiC) is so far considered as a promising wide band gap semiconducting material for high temperature, high frequency and high power electronic devices. In the present work we report on the structural characterisation of a 4H-SiC epitaxial layer grown by Chemical Vapour Deposition (CVD) in a horizontal, resistively heated, hot wall CVD reactor [1]. Stacking faults (SFs) are very common defects in all SiC polytypes, because of their small formation energy. Conventional transmission electron microscopy found in some areas of the studied material a very high density of defects, parallel to the basal hexagonal planes. High-resolution transmission electron microscopy (HRTEM) revealed that no isolated SFs appear. Instead the observed defects are three-dimensional ones, having the form of bands with a stacking sequence different than that of the 4H structure (…ABCBABCB…). These bands can be considered as the result of repeated SFs and (or) twin planes, within a distance of a few layers. Two types of bands were found very often to occur (“Figure 1a”): 1) An eight-bilayers (Si and C) band having the structure of a single unit cell of the 8H polytype, which has a stacking sequence: ABCABACB. 2) A fourteen-bilayers band. It contains three sub-bands, with four, six and four bilayers, respectively. Each sub-band has the cubic stacking sequence and is separated from the others by twin planes. In the electron diffraction patterns, taken from the highly defected regions of the specimens, satellite spots appear between the 4H reflections. Two sequences of spots were observed (“Figure 2”), denoting that at least two incommensurate modulated structures are locally created. HRTEM images reveal that the origin of these modulations is the quasi-periodic introduction of the defect bands. In the micrograph of “Figure 1b” a series of 8H single unit cells are seen, separated by a number (not always an integer one) of 4H unit cells. 1. 2.
T. Chassagne, A. Leycuras, C. Balloud, P. Arcade, H. Peyre and S. Juillaguet, Mat. Science Forum 457-460 (2004), p. 273. We kindly acknowledge that this work was performed in the frame of the MANSIC project (MRTN-CT-2006-035735), financed by EU.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 57–58, DOI: 10.1007/978-3-540-85226-1_29, © Springer-Verlag Berlin Heidelberg 2008
58
Figure 1. a) A HRTEM micrograph showing the presence of 8H and 14TC (14 layers twinned cubic) bands, having a different stacking sequence than the 4H matrix. b) A HRTEM micrograph, where the introduction of the 8H single unit cell bands occurs in a quasi-periodic way, giving rise to the appearance of satellite spots in the electron diffraction patterns.
Figure 2. Central [000l]* rows from electron diffraction patterns, denoting the local formation of SiC incommensurate modulated structures. The 4H reflections are indicated.
59
HRTEM study of AlN/3C-SiC heterointerfaces grown on Si(001) and Si(211) substrates T. Isshiki1, K. Nishio1, Y. Abe2, J. Komiyama2, S. Suzuki2, H. Nakanishi2 1. Kyoto Institute of Technology, Matsugasaki, Sakyo-ku, Kyoto 606-8585, Japan 2. Covalent Materials Corporation, 30, Soya, Hadano, Kanagawa 257-8566, Japan
[email protected] Keywords: AlN, SiC buffer layer, Interface structure, HRTEM
Epitaxial growth of nitride semiconductors on Si wafer is an important technique to develop electro-optical devices. However, a large lattice mismatch between Si and nitrides disturbs direct growth of defect-free nitride layer on Si substrate. Cubic SiC (3C-SiC), which can be formed directly on Si substrate [1], is attractive as a buffer layer to relieve the lattice mismatch. Nanoscopic information at interface between nitride and 3C-SiC is required to improve quality of growing nitride layer. In this work, interface structure between AlN and 3C-SiC buffer layer grown on Si(001) and Si(211) substrates is studied by high-resolution transmission electron microscopy (HRTEM). Specimen for cross-sectional HRTEM observation was prepared as following procedure. 3C-SiC buffer layer was grown on Si(001) and (211) substrates in a low pressure VPE reactor. After carbonization of Si substrates with C3H8 at 1200 °C, 3CSiC layer was grown with SiH4 and C3H8 at 1250 °C and 6.7 kPa in H2 atmosphere. AlN layer about 50-100 nm in thickness was deposited on the 3C-SiC at 1200 °C and 3.3 kPa in a low pressure MOVPE reactor using (CH3)3Al and NH3 with H2 carrier gas. On Si(001) substrate, 3C-SiC buffer layer grew with identical crystal orientation to the substrate with SiC(001) surface. On this surface, hexagonal AlN (h-AlN) didn’t grow directly, but cubic AlN(c-AlN) grew with pyramidal shape at the AlN/SiC interface within 10 nm in thickness, as shown in Figure 1. Since lattice mismatch between SiC(001) and c-AlN (001) is as small as 1.3%, c-AlN grew at first on the SiC(001) surface. However, due to phase instability of c-AlN, h-AlN grew on the four pyramidal c-AlN{111} planes immediately with h-AlN(0001) parallel to c-AlN{111}. As a result, growth layer was composed of h-AlN domains being in twin relation. A Si(211) substrate is restructured spontaneously to undulant structure of Si(111) and Si(200) facets during carbonized process [2]. Therefore, nano-facet structure of flat SiC(111) and unclear SiC(200) also appeared at surface of growing 3C-SiC buffer layer, as shown in Figure 2. On the flat SiC(111) facet, h-AlN grew coincidently with (0001) plane parallel to the facet. On the other hand, small voids and (11, 01) twin crystal were observed near the SiC(200) facet. Stacking faults propagating from the SiC layer were absorbed by the voids and didn’t propagate in h-AlN layer. Generation of new defect at the interface is hardly observed except twin boundary mentioned above. 1.
S. Nishino, H. Suhara, H. Ono and H. Matsunami, J. Appl. Phys. 61 (1987) 4889
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 59–60, DOI: 10.1007/978-3-540-85226-1_30, © Springer-Verlag Berlin Heidelberg 2008
60
2.
T. Nishiguchi, Y. Mukai, M. Nakamura, K. Nishio, T. Isshiki, S. Ohshima and S. Nishino, Materials Science Forum 457-460 (2004) 285.
Figure 1. HRTEM image at interface of AlN grown on SiC(001) / Si(001).
Figure 2. HRTEM image at interface of AlN grown on SiC(111) and SiC(200) / Si(211).
61
Electron microscopy of GaAs/AlGaAs quantum cascade laser A. Łaszcz, J. Ratajczak, A. Czerwinski, K. Kosiel, J. Kubacka-Traczyk, J. Muszalski, M. Bugajski and J. Kątcki Institute of Electron Technology, Al. Lotników 32/46, 02-668 Warsaw, Poland
[email protected] Keywords: transmission electron microscopy, quantum cascade laser, GaAs, AlGaAs
The quantum cascade laser (QCL) is based on a different principle comparing to bipolar semiconductor lasers, because it uses only one type of the charge carriers – electrons and therefore is called an unipolar laser. The essence of the QCL is an operation like an electronic waterfall. Electrons cascade down a series of identical energy steps built into the material during crystal growth, emitting a photon at each step as opposed to diode lasers which emits only one photon over the similar cycle. The other aspect of the QCL is the possibility of emission over a wide range of wavelengths using the same combination of materials in the active region [1]. The use of GaAs/AlGaAs heterostructures for preparation of unipolar laser has been demonstrated by Sirtori et al. in 1998 [2] and it was not restricted to one material system. We report electron microscopy study of GaAs/AlGaAs QCL structure fabricated by the Molecular Beam Epitaxy (MBE) technique. The QCL was designed according to the scheme described in Table I. The studies focused on MBE technology verification and precision of realization of layer’s thicknesses in the active region of the QCL. Transmission electron microscopy (TEM) observation showed a repeatability of modules in the active region (30x16 GaAs/AlGaAs layers, Figure 1a). However, an increase of each module thickness with reference to the initial assumption (Table I) has been observed. Intended thickness of one module was 45.3 nm. The one determined by TEM measurements equals 48.9 nm (Figure 1b). The ratio of measured to desired thickness of layers is 1.079. TEM results were confronted with X-ray diffraction (XRD) analysis of layer thickness in the active region. XRD results showed that the ratio of measured to desired thickness of layers is 1.075 [3]. The difference between thickness determined by both methods is only 0.4%. 1. 2. 3. 4.
J. Faist, F. Capasso, D.L. Sivco, C. Sirtori, A.L. Hutchinson and A.Y. Cho, Science 264 (1994), p. 553. C. Sirtori, P. Kruck, S. Barbieri, P. Collot, J. Nagle, M. Beck, J. Faist and U. Oesterle, Applied Physic Letters 73, No. 24 (1998), p. 3486. K. Kosiel, M. Bugajski, J. Muszalski, J. Kubacka-Traczyk, J. Ratajczak, A. Łaszcz, P. Romanowski, R. Mogilinski, J. Gaca and M. Wójcik, Design and MBE Growth, Optimization of Mid-Infrared Quantum Cascade Laser Structures - Int. Conf. on Semiconductor Materials and Optics (SMMO 2007).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 61–62, DOI: 10.1007/978-3-540-85226-1_31, © Springer-Verlag Berlin Heidelberg 2008
62
Table I. Scheme of GaAs/AlGaAs quantum cascade laser.
Figure 1. TEM images of: (a) active region of quantum cascade laser (30x16 GaAs/AlGaAs layers) and (b) high magnification of the first module of the active region with 16 GaAs/AlGaAs layers.
63
Solving the crystal structure of highly disordered Sn3P4 by HRTEM O.I. Lebedev, A.V. Olenev, G. Van Tendeloo EMAT, University of Antwerp, Groenenborgerlaan 171, B2020 Antwerpen, Belgium
[email protected] Keywords: crystal structure, disordering, HRTEM
Disordered narrow-gap semiconductors have recently been investigated in the context of a search for new thermoelectric materials. Sn3P4 is a narrow-gap semiconductor exhibiting a relatively high thermal conductivity of about 8 W m–1 K–1. Upon cooling to 150 K it undergoes a remarkable transition from n-type conduction to p-type conduction. The crystal structure of Sn3P4 long remained unsolved since its discovery in 1920. In order to check possible superstructure formation Sn3P4 has been investigated by TEM. ED patterns for Sn3P4 along the main zones are shown in Fig.1. Remarkably, only the brighter spots in the [0001] ED pattern (Fig.1a) can be indexed using the X-ray single crystal data. On the [–1100] and [01–10] ED patterns (Fig.1b and c, respectively) streaks along the c* axis are clearly present. Along the [0001] zone these streaks intersect the plane and produce sharp spots (Fig. 1a, d) (marked by squares and triangles). To understand the nature of the streaks HRTEM was performed along [01-10] (Fig.2). The streaks are also clearly observed on the FT, indicating that the origin of the streaks is captured in the image. The image itself has a number of peculiarities: the rows of dots along the a axis are arranged in such a way that a bright dot is followed by a dim dot. The X-ray data unambiguously showed that while the sites of the tin atoms are fully occupied, the phosphorus atoms, joined into dumbbells, are disordered in such a way that only one out of four dumbbells can be present in each block of the structure. Consequently, the contrast modulation, observed in Fig.2a is most probably associated with a short range ordering of P atoms along the a axis. Good agreement between the experimental and the calculated image may be achieved by introducing a partially ordered model (shown in Fig.2c), in which disordered P24– dumbbells alternate along the a direction with partially ordered fragments. In these fragments, only two out of four possible dumbbells remain intact, the third is broken leaving a separate phosphorus atom, and the fourth is missing. One can see (Fig.2a marked by white frames) that modulated rows of dots in some cases are shifted along the c direction. This shift is random, which means that disordered and partially ordered phosphorus fragments irregularly alternate along the c axis as shown in Fig.2c. This irregularity leads to the formation of streaks in the [–1100] and [01–10] ED patterns. An image of the basic Sn3P4 structure can be obtained by applying a Bragg-mask filter for only the basic spots (correspond to the brighter reflections on the ED pattern). Inverse FT results in the image shown in Fig. 2b. In this case, a uniform intensity distribution in the rows of bright dots is achieved. An image calculated on the base of the X-ray structure S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 63–64, DOI: 10.1007/978-3-540-85226-1_32, © Springer-Verlag Berlin Heidelberg 2008
64
refinement (inset Fig. 2b) perfectly fits and shows that the rows of bright dots correspond to the positions of Sn(1) in the average crystal structure.
Figure 1. ED patterns along the major zones of Sn3P4
Figure 2. (a) [01-10] HRTEM image of Sn3P4 and its corresponding FT pattern. The SnP block stacking along the c axis is marked with white quadrangles. The modulation along the Sn layer is marked by white arrows; (b) filtered HRTEM image of (a). Only the basic spots were included in the mask; (c) proposed structure model of the disordered structure. Simulated images based on a disordered model (c) and the ordered model (X-ray data) are given as inset in (a) and (b).
65
Determination of In-distribution in InGaAs quantum dots D. Litvinov1, H. Blank1, R. Schneider1, D. Gerthsen1 and M. Hetterich2 1. Laboratorium für Elektronenmikroskopie, Universität Karlsruhe, D-76128 Karlsruhe 2. Institut für Angewandte Physik, Universität Karlsruhe, D-76128 Karlsruhe
[email protected] Keywords: quantum dot, InGaAs, TEM
We investigated InAs/GaAs quantum dot (QD) layers by quantitative transmission electron microscopy (TEM) and photoluminescence (PL) spectroscopy. To achieve the highest possible In-concentration in the QDs and maximum QD sizes, InAs QD layers with a nominal thickness of 2.6 ML were grown by molecular-beam epitaxy on GaAs (001) with a low deposition rate of 0.006 monolayers (ML)/sec at 500 °C. To reduce the strong In-segregation, which is observed in InAs/GaAs heterostructures during the growth of the GaAs cap layer, the InAs QD layers were capped by InGaAs with a nominal thickness of 6 nm and finally by a GaAs cap layer with 30 nm thickness. The influence of different In-concentrations x in the InxGa1-xAs cap layer (x = 0, 0.05, 0.1, 0.15, 0.2 and 0.25) on the structural and optical properties was studied. The Indistribution in the QD layers was determined with the composition evaluation by lattice fringe analysis technique (CELFA) [1] which is based on the chemical sensitivity of the (002) reflection for the sphalerite structure. The measured In-concentration in the QDs is artificially lowered due to the averaging effect of a TEM sample with finite thickness and the three-dimensional nature of the QDs embedded in a matrix with lower Inconcentration. A post-processing procedure was developed and applied to the raw CELFA data to determine the real In-concentration in the QDs. We combine conventional, quantitative high-resolution and high-angle annular darkfield scanning transmission electron microscopy of plan-view and cross-sectional samples to determine the shape and size of the quantum dots. The shape of QDs, which is a truncated pyramid with square bases along the <100> directions and with {101} facets, is essentially independent of the cap-layer composition. To determine the TEM specimen thickness in the QD region, a tilt series of cross-section images was taken with the chemically sensitive (200) reflection. For the CELFA evaluation, only QDs were chosen which are fully embedded in the Ga(In)As cap layer, i.e. without any sectioning due to TEM specimen preparation. For the post-processing we calculate a function which - applied to the CELFA data multiplies values of the local In-concentration by the quotient of the local thickness of the sample and the local thickness of the QD. Figures. 1a,c are color-coded maps of the In-concentration obtained with CELFA for the samples capped by GaAs and In0 2Ga0 8As. For comparison, Figures. 1b,d display the corresponding maps after the post-processing with a other color scale. The thicknesses of the TEM specimens according to the tilt series are 33 nm for the GaAs-capped QD and 38 nm for the In0 2Ga0 8As-capped QD. Since the correction was only applied to the QD region, the wetting layer is not visible in the corrected maps. The imaging was carried out with the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 65–66, DOI: 10.1007/978-3-540-85226-1_33, © Springer-Verlag Berlin Heidelberg 2008
66
(200) lattice fringes (perpendicular to the substrate/layer interface), which are less affected by lattice plane bending in contrast to the (002) lattice planes parallel to the growth direction. The white triangles indicate the approximate QD shape and size. The lateral size of the QDs increases with the In-concentration in the cap layer from about 20 nm for the sample with x = 0 to 24 nm for the island with x = 0.2, while the QD height increases only slightly from 6.8 to 7.3 nm. The white arrows mark the maximum of the In-concentration within the QDs which shifts upward after the correction. The determination of the composition of the layers after post-processing shows that the Inconcentration in the QDs increases in growth direction and reaches values up to 90 %. Redistribution of indium during the InGaAs cap layer growth leads to a decrease of the In-concentration in the cap layer with respect to the nominal In-concentration. The observed red shift of the PL peak with increasing In-concentration in the cap layer is attributed to the enlargement of island size and the change of the strain in the QD layers caused by the misfit between InAs and the cap layer. 1. 2.
A. Rosenauer, Transmission Electron Microscopy of Semiconductor Nanostructures - An Analysis of Composition and Strain (Heidelberg, Springer) Springer Tracts in Modern Physics (2003), 182 p. This work has been performed within the project A.2 of the DFG Research Center for Functional Nanostructures (CFN). It has been further supported by a grant from the Ministry of Science, Research and the Arts of Baden-Württemberg (Az: 7713.14-300).
Figure 1. Colour-coded In-concentration maps obtained with CELFA using the (200) reflection in samples capped by GaAs (a,b) and In0 2Ga0 8As (c,d) before (left-hand side) and after post-processing of the CELFA data (right-hand side). The white triangles delineate the QD shape.
67
Nanoanalytical investigation of the dielectric gate stack for the realisation of III-V MOSFET devices. P. Longo1, A.J. Craven1, M.C. Holland2 and I.G. Thayne2 1. Department of Physics and Astronomy, University of Glasgow, G12 8QQ, UK 2. Department of Electrical & Electronics Engineering, University of Glasgow, G12 8LT, UK
[email protected] Keywords: TEM, EELS, STEM, compositional analysis, MOSFET, gallium arsenide
Planar Si MOSFET technology using Si(ON) is rapidly approaching its theoretical limit and the search for new material is essential. n-type GaAs has a mobility 5 times higher than Si [1]. This makes it a suitable candidate for MOSFETs devices. So far, GaAs has not been used for practical MOSFETs because of the difficulties of making a good dielectric oxide layer in terms of leakage current and unpinned Fermi Level. Using processes pioneered by Passlack et al. [2], dielectric gate stacks consisting of a template layer of amorphous Ga2O3 followed by amorphous GdGaO have been grown on GaAs substrates. Careful deposition of Ga2O3 can leave the Fermi Level unpinned. The introduction of Gd is important in order to decrease the leakage of current. Electron energy-loss spectroscopy (EELS), carried out in a nano-analytical electron microscope, has been shown to be an excellent method to characterise Ga2O3/GdGaO dielectric stacks [3]. Spectrum imaging (SI) uses computer control to position the electron beam and to record one or more spectra at each point, building up an Ndimensional data set. It is also possible to quantify the amount of each element present, with extremely high spatial resolution. Such approach has been applied to the characterization of a number of GaAs/Ga2O3/GdxGa0 4-xO0 6 systems where x is the Gd atomic fraction. The thickness of the GdGaO layer varies from 9nm up to 60nm. In general, the Gd concentration decreases with the distance from the substrate. However we have observed an increase in one case where the peak Gd concentration was 36%. For Gd target concentration of 20%, the films are normally amorphous. As the Gd concentration increases, crystallisation can start to occur at >25%. However we have also observed the start of crystallisation at lower Gd concentration under specific growth conditions. “Figure 1” shows a high-resolution TEM bright field image of the GaAs/Ga2O3/GdGaO dielectric gate stack where the highest Gd content detected is 36%. The high Gd concentration causes the partial crystallisation of the GdGaO layer as shown in Figure 1. The Fourier Transform inset in “Figure 1” also shows the preferred orientation of the lattice structure in the GdGaO layer. XRD analysis has confirmed the presence of crystalline Gd2O3 in the GdGaO layer. The avoiding crystallisation is an important factor during the growth of the dielectric stack for MOSFET devices. The optimum conditions in terms of device properties are when the GGO layer is completely amorphous. “Figure 2” shows the elemental composition across the GdGaO layer. The
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 67–68, DOI: 10.1007/978-3-540-85226-1_34, © Springer-Verlag Berlin Heidelberg 2008
68
thickness profile ranges from 0.22 down to 0.1t/λ. The Gd concentration slightly increases on moving away from the Ga2O3 layer and reaches the highest value in the area at 22nm. On the hand the O concentration appears to be slightly below 60%. However in the region in the top surface of the GdGaO layer the O concentration increases significantly. A sharp drop of t/λ is seen in the region where the O concentration increases. Thus the increase in the O concentration is likely to be due to the presence of surface layers with modified composition whose effects become stronger as the sample gets very thin. 1. Wang YC, Hong M., Kuo JM., Kwo J., Mannaerts JP, Chen YK and Cho Y., IEEE, Electron Device Letters 20, 457, 1999 2. Passlack M, Yu Z, Droopad R, Bowers B, Overgaard C, Abrokwah J, and Kummel AC, J Vacuum Science & Technology B17, 1, 49-52, 1999 3. Longo P, Craven AJ, Scott J, Holland MC and Thayne IG proceedings of MSM XV, 2007 4. Authors would like to acknowledge EPSRC support under grant EP/F002610 and Mr B. Miller for TEM specimen preparation.
GdGaO
Ga2O 3 GaAs Figure 1. High-resolution TEM bright field image of the GaAs/Ga2O 3/GdGaO dielectric gate stack. The GdGaO layer is partly crystalline with preferential orientation, as shown in the inset Fourier Transform. 0.3 0.25
50
0.2
40 30
0.15
20
0.1
10
0.05
0
Ga% t/lambda
atomic percent
60
Gd% O% t/lambda
0 0
10
20
30 nm
40
Figure 2. Elemental concentrations across the GdGaO layer. The 0 on the x-axis represents the main boundary between the Ga2O 3 template layer and the GdGaO. The thickness profile is also shown.
69
Phase mapping of uncapped InN quantum dots J.G. Lozano1, M. Herrera2, R. García1, N.D. Browning2,3, S. Ruffenach4, O. Briot4 and D. González1 1.Departamento de Ciencia de los Materiales e Ingeniería Metalúrgica y Química Inorgánica, Universidad de Cádiz, Apdo 40, E-11510 Puerto Real (Cádiz), Spain 2. Department of Chemical Engineering and Materials Science, University of California-Davis, One Shields Ave, Davis, CA 95616, USA 3. Chemistry, Materials Science and Life Sciences Directorate, Lawrence Livermore National Laboratory, 7000 East Avenue, Livermore, CA 94550, USA 4. Groupe d’Etudes des Semiconducteurs, UMR 5650 CNRS, Place Eugène Bataillon, Université Montpellier II, 34095 Montpellier, France
[email protected] Keywords: Indium Nitride, Indium Oxide, HRTEM, Phase mapping
InN has in recent times attracted much attention due to its outstanding electronic properties and recently set low band gap of 0.7 eV [1]. However, it has been the nitride that has generated higher controversies about its fundamental parameters, due to the difficulties associated to its growth and to the application of standard measurement techniques developed for other III-V materials. Many of these variations in the measured values are ascribed to oxygen contamination [2], either during the growth process, either as a simple natural aging process. The aim of this work is to obtain maps of the location of the different phases inside the InN nanostructures, by using high resolution transmission electron microscopy (HRTEM) combined with the geometric phase (GP) algorithm [3]. The samples were grown by metalorganic vapour phase epitaxy [4] onto sapphire substrates, using a thick (1 μm) GaN buffer layer grown at a temperature of 1000º C; on top of which InN quantum dots were grown at a temperature of 550º C. The experimental analysis were carried out in a JEOL 2010FEG and JEOL 2500 transmission electron microscopes operating at 200 kV. Figure 1(a) shows a cross sectional HRTEM of an InN QD, and Figure 2(b) its associated Fast Fourier Transform (FFT). In the last, several phases can be distinguised: wurtzite InN oriented along the <11-20> zone axis, two bcc-In2O3 crystals oriented along the <110> pole and rotated 180º around the growth direction one with respect to each other and a InN zincblende phase, whose main spots share position with the In2O3 phases. To reconstruct the crystal position we used the GP algorithm, and the results are shown in Figure 2. It can be seen that the hexagonal InN phase has disappeared in the areas near the surface shrinking to the centre of the QD. Additionally, the two sets of inclined fringes correspond cubic phases (zinc-blende InN and bcc-In2O3). Therefore, in the final configuration cubic phases form a surrounding layer that envelops a core of InN-w. Although In2O3 constitutes the mainly component of the cubic regions, the presence of InN-zb is also reported
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 69–70, DOI: 10.1007/978-3-540-85226-1_35, © Springer-Verlag Berlin Heidelberg 2008
70
1. 2. 3. 4.
A.G. Bhuiyan, A. Hashimoto, A. Yamamoto, J. Appl. Phys. 94, 2779 (2003) M. Yoshimoto, H. Yamamoto, W. Huang, H. Harima, J. Saraie, A. Chayahara and Y. Horino Appl. Phys. Lett., 83, 3480 (2003) O. Briot. B. Maleyre, S. Ruffenach, Appl. Phys. Lett. 83, 14 (2004) M.J. Hÿtch, E. Snoeck and R. Kilaas, Ultramicroscopy 74 (1998) 131
Figure 1.(a) X-HRTEM micrograph of an uncapped InN QD taken along the <11-20> pole. In the inset, FFT of this micrograph (b) Diffraction patterns simulated over the FFT image where yellow triangles correspond to InN-w, white and pink squares correspond to both InN-zb grains and red and green circles simulate the In2O3 grains.
Figure 2. Numerical moiré fringes mappingof the uncapped QD taking as reference the spot g11-2 spot of the In2O3 crystals. The radius of the Bragg mask was chosen to include the {222} spots of the FFT images (see blue circle in Fig.1b)
71
STEM investigations of (In,Ga)N/GaN quantum wells P. Manolaki1, I. Häusler1, H. Kirmse1, W. Neumann1, P. Vennéguès2, P. De Mierry2 and P. Demolon2 1. Humboldt-Universität zu Berlin, Institut für Physik, AG Kristallographie, Newtonstrasse 15, D-12489 Berlin, Germany. 2. Centre de Recherche sur l'Hétéro-Epitaxie et ses Applications, rue Bernard Grégory, 06560 Valbonne, France
[email protected] Keywords: Quantum wells, (In,Ga)N, STEM
Nanostructures of III-N semiconductors have a great commercial potential due to their optoelectronic properties. The structural and chemical characteristics of such structures determine the performance of the light-emitting devices. Transmission electron microscopy can be used to determine these characteristics at a nanometer scale. Nanostructures were generated by metal organic chemical vapour deposition on sapphire (0001). First a GaN buffer layer doped with Si was grown on the substrate. In a second step 5 (In,Ga)N/GaN multilayers of a nominal In content of 8.5 at. % were grown. The nominal thickness of the (In,Ga)N layers was 2.6 nm separated by a 22 nm thick GaN barrier layer. The structure was capped by a 200 nm thick GaN layer doped with Mg. For the p-contact a double layer consisting of 5 nm Ni and 5 nm Au was deposited. The (In,Ga)N quantum wells (QWs) were grown at a temperature of 755 °C, whereas the GaN barriers were grown at 975 °C. The sample was prepared for TEM by mechanical preparation comprising formatting, mechanical polishing, dimpling, and finally ion milling. Structural and chemical analysis was performed on a TEM/STEM JEOL JEM2200FS operating at 200 kV. The instrument is equipped with a high-angle annular dark-field (HAADF) detector and an energy dispersive X-ray (EDX) spectrometer. The minimum probe size in STEM mode is 0.14 nm. In the composition-sensitive STEM HAADF image of the Figure 1 the 5 QWs as well as the Ni/Au contact layer appear brighter than the substrate, the buffer layers and the cap layer, because they contain elements of a higher atomic number. In addition, Figure 1 shows a number of screw and edge dislocations originating from the buffer. Figure 2, which is a magnification of the marked area of Figure 1, evidences that the individual (In,Ga)N layers exhibit inhomogeneous intensity as well as varied thickness. Figure 3 is a STEM image of another area of the sample, where just below the contact layer trapezoidal pits are visible. However, they are not initiated at threading dislocations. The results of the analysis of the chemical composition of the (In,Ga)N/GaN QWs and of the barriers by EDXS show an In content of 4 to 8 at% which is below the nominal value of 8.5 at% (see Figure 4). The results of the EDX line scan along the first QW are given in Figure 5, verifying a compositional inhomogeneity. The In composition for the QWs can be also evaluated by using strain analysis on high-resolution TEM images of the (In,Ga)N QWs as described in [1]. S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 71–72, DOI: 10.1007/978-3-540-85226-1_36, © Springer-Verlag Berlin Heidelberg 2008
72
1. 2.
P. Ruterana, S. Kret and M. A. Poisson, Mater. Sci. Eng. B 93, (2002), p. 185. This work was financially supported by the Marie Curie Research Training Network PARSEM (contract No.: MRTN-CT-2004-005583).
Figure 1. STEM HAADF overview of the QW, of the contact layer and of dislocations, respectively
Figure 2. Magnification of the framed area of Figure 1
Figure 4. EDX spectrum of the line scanning across the layers (see green arrow on Figure 2)
Figure 3. STEM overview of the QWs and the contact layer of another area of the sample
Figure 5. EDX spectrum of the line scanning along the first QW (see blue arrow on Figure 2)
73
Defects in m-plane GaN layers grown on (100) γ-LiAlO2 A. Mogilatenko1, W. Neumann1, T. Wernicke2, E. Richter2, M. Weyers2, B. Velickov3 and R. Uecker3 1. Institut für Physik, Humboldt Universität zu Berlin, Newtonstr. 15, 12489 Berlin, Germany 2. Ferdinand-Braun-Institut für Höchstfrequenztechnik, Gustav-Kirchhoff-Str. 4, 12489 Berlin, Germany 3. Institut für Kristallzüchtung, Max-Born-Str. 2, 12489 Berlin, Germany
[email protected] Keywords: GaN, thin films, crystal defects
In the last years (100) γ-LiAlO2 was used as an alternative substrate for GaN epitaxy [1, 2]. In contrast to the commonly used commercial substrates (100)LiAlO2 allows a nearly lattice-matched growth of both polar c-plane and non-polar m-plane oriented GaN layers. The m-plane oriented GaN layers show absence of internal polarisation fields along the growth direction [1-1.0]GaN which is advantageous for fabrication of optoelectronic devices with high performance [2]. Furthermore, LiAlO2 decomposition at elevated substrate temperatures [3] leads to spontaneous separation of the substrate from thick GaN layers during post-growth cooling down [1, 4]. This allows the preparation of freestanding GaN layers, which can be used as substrates for subsequent GaN homoepitaxy. In the present study we applied transmission electron microscopy (TEM) to investigate the structure of m-plane GaN layers grown on LiAlO2 by metal organic vapour phase epitaxy (MOVPE) process. Plan-view diffraction contrast analysis shows the presence of different types of defects. The m-plane GaN layers contain a large number of basal plane stacking faults (BSF) which are visible in the bright-field image obtained with a (10-10)GaN reflection (Figure 1a). The nature of the stacking faults was determined in cross-section (Figure 2a). According to high resolution TEM analysis they are intrinsic stacking faults of I1 type (Figure 2b). This defect corresponds to the following stacking sequence: …ABABABCBCBC…, where each capital letter represents a layer consisting of a Ga-N atom pair. This stacking fault is characterized by a displacement vector R = {1/3[1-1.0] + ½[00.1]}. Additionally, the layers contain a complicated net of boundaries which are visible in the bright-field image obtained with a (0002)GaN reflection (Figure 1b). According to the thickness fringes in Figure 1b it seems that this net of boundaries consists of planar defects located on a number of GaN planes, which are inclined to the growth direction. These defects are characterised by a displacement vector R arranged parallel to [00.1]GaN. Cross-sectional analysis proved the presence of grain boundaries at {10-10}, {1-102} as well as {1-103}GaN planes. The inclined boundaries act as additional nucleation sites for the BSF formation (Figure 2c).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 73–74, DOI: 10.1007/978-3-540-85226-1_37, © Springer-Verlag Berlin Heidelberg 2008
74
1. 2. 3. 4.
H.P. Maruska, D.W. Hill, M.C. Chou, J.J. Gallagher, B.H. Chai, Opto-electronics Rev. 11 (2003), p. 7 P. Waltereit, O. Brandt, A. Trampert, H.T. Grahn, J. Menniger, M. Ramsteiner, M. Reiche, K.H. Ploog, Nature 406 (2000), p. 865 A. Mogilatenko, W. Neumann, E. Richter, M. Weyers, B. Velickov, R. Uecker, J. Appl. Phys. 102 (2007), p. 023519 E. Richter, Ch. Hennig, U. Zeimer, M. Weyers, G. Tränkle, P. Reiche, S. Ganschow, R. Uecker, K. Peters, Phys. Stat. Sol. (c) 3 (2006), p. 1439
Figure 1. Plan-view bright-field images of m-plane GaN layers deposited by MOVPE. The images were obtained under two-beam conditions with (a) (10-10)GaN reflection and (b) (0002)GaN reflection. Basal plane stacking faults and a net of grain boundaries are visible in (a) and (b), correspondingly.
Figure 2. (a) Cross-sectional bright-field image of m-plane GaN layer shows the presence of BSF and defects which are inclined to the [1-1.0]GaN growth direction. (b) High-resolution TEM image of a BSF proves the layer sequence:…ABABCBC… (c) A zigzag shaped grain boundary in m-plane GaN acts as a nucleation site for the BSF formation.
75
Improvements on InP epilayers by the use of monoatomic hydrogen during epitaxial growth and successive annealing F.M. Morales1, A. Aouni2, R. García1, P.A. Postigo3, C.G. Fonstad4, S.I. Molina1 1. Departamento de Ciencia de los Materiales e Ingeniería Metalúrgica y Química Inorgánica, Universidad de Cádiz, 11510 Puerto Real, Cádiz, Spain 2. Faculté de’Sciences et Techniques, Université Abdelmalek Essadi, BP 416 Tanger, Morocco 3. Instituto de Microelectrónica de Madrid, Centro Nacional de Microelectrónica, CSIC, Isaac Newton 8, PTM Tres Cantos, 28760, Madrid, Spain 4. Department of Electrical Engineering and Computer Science, and Microsystems Technology Laboratory, MIT, Cambridge, Massachusetts 02139, USA fmiguel
[email protected] Keywords: InP on GaAs, MBE, TEM
InP has demonstrated advantages for optoelectronics and wireless applications but there is still a lack of products which offer big InP surfaces for its microelectronics integration. The heteroepitaxy of InP films on cheap and large GaAs substrates would be an appropriate solution for this necessity since bulk InP wafers are available only in small sizes and at high prices [1]. In this way, the challenge for InP growers focuses on finding the best alternatives for avoiding the negative effects produced by the lattice mismatches and the differences in the thermal expansion coefficients between active InP films and substrate materials. Beyond the use of buffer intermediate layers between InP and GaAs, the technique of direct growth of InP on GaAs using monoatomic hydrogen has recently demonstrated excellent results. Compared to homoepitaxial InP layers grown under the same conditions, H-assisted heteroepitaxial InP showed enhanced optical properties. Hydrogen helped to a raise on the critical thickness of 40 times larger than that expected for such a high misfit on InP/GaAs [2]. The characterization of high-quality InP epilayers fabricated by low temperature (200-480ºC) solid-source molecular beam epitaxy on (001) GaAs is reported in this work. The optimized two-step production process is firstly assisted by monoatomic hydrogen in the earliest stages of the molecular beam epitaxy growth. After growth, some samples have been rapid-thermal annealed (RTA). Selected area electron diffraction (SAED) studies confirm that the InP layers are always well heteroepitaxially placed as indicated by perfect alignments between GaAs and InP diffraction lattice spots. It is concluded by the analyses of the diffraction patterns and the study of interfaces in highresolution transmission electron (HRTEM) micrographs that the zinc-blende InP is almost strain relaxed. These images allowed observing misfit dislocations located just at the interface and formed after the critical thickness was reached during the growth. Moreover, two other main kind of structural defects were observed from diffractioncontrast transmission electron micrographs (DC-TEM), both typical of cubic crystals: stacking faults (SF) and tangled threading dislocations (TDs). These imperfections are
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 75–76, DOI: 10.1007/978-3-540-85226-1_38, © Springer-Verlag Berlin Heidelberg 2008
76
mostly confined to a region of less than 500 nm above the InP/GaAs interface (due to interfacial strain) and their densities decrease monotonically as they approach the surface of thee ~2 μm thick InP films (auto-annihilation and decreased stress). The TDs appear irregularly spread across the f and are revealed with g vectors parallel to <220> or <400> directions on cross-sections. However, planar defects did not appear in the samples with higher H doses and the interface region looks cleaner of imperfections. As a rule, it is found a diminution on the density of TDs on the layers when either H or RTA is used (Fig. 1). For improved samples (H+RTA), the TD density was measured to be on the range of 108 cm-2, which is a good result compared to state of the art InP epilayers [3]. However, comparable quantities of such line defects have demonstrated to improve electrical and optical properties by acting as a gettering network located beneath the device zone on InP/GaAs based high-electron mobility transistors [4]. 1 2 3 4
R. Szweda, III-Vs Review, 13, 55 (2000) P. A. Postigo, F. Suarez, A. Sanz-Hervás, J. Sangrador and C. G. Fonstad, J. Appl. Phys. 103, 013508 (2008). K.-F. Yarn, C.-I Liao and C.-L. Lin, Crystallographic Reviews, 12, 47–80 (2006). Y. Liu and H. Wang J. Appl. Phys. 100, 034505(2006)
Figure 1 HRTEM micrographs of the InP layer showing a SF (a) and a structure clean of defects (b). TDs at the surface of the optimum sample (i. e. higher content of H during growth and subsequent RTA) (c). SAED pattern showing both GaAs and InP aligned related spots without contrasts associated to defects (d). CDTEM micrographs (g=002) of the InP layers for conditions: No H and No RTA (e); High H and No RTA (f); Medium H + RTA (g) and; High H + RTA (h).
77
Study of microstructure and strain relaxation on thin InXGa1-xN epilayers with medium and high In contents F.M. Morales1, J.G. Lozano1, R. García1, V. Lebedev2,3, S. Hauguth-Frank2, V. Cimalla2,3, O. Ambacher3, D. González1 1. Departamento de Ciencia de los Materiales e Ingeniería Metalúrgica y Química Inorgánica, Facultad de Ciencias, Universidad de Cádiz, 11510 Puerto Real Cádiz, Spain 2. Institute of Micro- and Nanotechnologies, Technical University Ilmenau, 98693 Ilmenau, Germany 3. Fraunhofer Institute for Applied Solid State Physics, Tullastrasse 72, D-79108 Freiburg, Germany fmiguel
[email protected] Keywords: InGaN, High resolution TEM, Strain
GaN and InGaN with a high content of Ga became the most important semiconductors for light emission and detection in the visible and the near UV spectral regions. On the other hand, the fabrication of InGaN epilayers with medium and high concentration of In is still not well developed. However, the control of the growth of alloys within this In-rich range would give rise to expand the optical activity of InGaN till the near IR. Recently, the compositional dependencies of photoconductivity and electron transport properties for metal-semiconductor-metal photodetectors based on Inrich InGaN ultra-thin films were studied [1]. There, the electron density profiles and low-field mobilities for different compositions of InGaN were calculated. It was demonstrated that in contrast to bulk InN exhibiting a dominating surface electron accumulation, the free electrons in ultra-thin InxGa1-xN/GaN (0.5<x<1) heterostructures tend to accumulate mostly at the buried InGaN/GaN interface. In this work we report on the fabrication and studies of high structural quality wurtzite InGaN nanolayers grown on top of Al2O3/AlN/GaN epitaxial substrates within this unexplored range of compositions of medium and high In concentrations (0.4<x<0.8). The epilayers are single-crystalline and did not show appreciable phase segregation or compositional modulation. Electron and X-ray diffraction were used for an accurate estimation of the actual a- and c-lattice parameters. The thin InGaN layers present a tetragonal distortion (i. e. strained by biaxial compressive stress) which decrease monotonically as the In content is higher for the same film thickness. This effect was also confirmed by the observation of high-resolution transmission electron micrographs. Therefore, the accurate composition of InGaN alloys should be assessed not only by diffraction methods, but by chemical analysis to serve as an independent reference, since for biaxial compressed InGaN, Vegard’s law interpolations lead to systematic overestimations of In compositions. For this reason, the technique of energy dispersive X-ray spectroscopy in scanning transmission electron microscopy mode was carried out for the best measurement of In/Ga compositions, in the same regions, where
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 77–78, DOI: 10.1007/978-3-540-85226-1_39, © Springer-Verlag Berlin Heidelberg 2008
78
selected area electron diffraction patterns were registered. Once correlated the perpendicular and the in-plain strain with respect to each composition, it is concluded that the elastic constants of the studied ternary alloys follow a linear trend between those of GaN and InN binary compounds. These results have been confronted to and supported by measurements of the strain state in low and very high In concentration InGaN/GaN heterosystems by different research teams. Moreover, we propose a model of the critical thicknesses, which delimitates a transition state between pure pseudomorphic and completely relaxed layers as the In concentration on InGaN/GaN varies in the complete range of compositions (0<x<1). Our observations agree with the linear relationship between lattice spacing and the alloy composition demonstrated for free-standing InGaN (i. e. nanowires [2] or non-coalesced island growth) and denies the idea that this relation is subjected to a noticeable bowing parameter. 1. 2.
V. Lebedev, V. M. Polyakov, S. Hauguth-Frank, V. Cimalla, Ch. Y. Wang, G. Ecke, F. Schwierz, A. Schober, J. G. Lozano, F. M. Morales, D. González and D. González, J. Appl. Phys. 103, in press (2008). T. Kuykendall, P. Ulrich, S. Aloni and P. Yang, Nature Materials 6, 951 (2007)
79
Convergence of microscopy techniques for nanoscale structural characterization: an illustration with the study of AlInN A. Mouti1, S. Hasanovic1, M. Cantoni1, E. Feltin2, N. Grandjean2, P. Stadelmann1 1. Interdisciplinary center for electron microscopy (CIME), EPFL, Lausanne, Switzerland 2. Laboratory of Advanced Semiconductors for Photonics and Electronics (LASPE), EPFL anas
[email protected] Keywords: III nitrides, TEM, SEM, AFM, Alloy, Dislocation, InAlN, AlInN, GaN
AlInN is a wide band gap group III nitride alloy, it is gaining interest nowadays because of its ability to be lattice matched to GaN, thus reducing defect creation. Recent research [1] has allowed the growth of good quality AlInN /GaN heterostructures on sapphire. However, AlInN is quite a complex alloy to grow and characterize, partly because of the high difference in ionic radii between Aluminum and Indium. The high dislocation density inherited from the lattice mismatch between GaN and Sapphire adds considerable complexity. Therefore, many physical phenomena can occur in this alloy, making it an interesting material for the microscopist. We present a broad structural study of AlInN to characterize its order and disorder, defects, interfaces, e-beam sensitivity. Weak beam dark field has been used to characterize dislocations and has been coupled with AFM to study surface pits “Figure 1”. EDX microanalysis in TEM was used to quantify compositional fluctuations with a 0.5% accuracy and a 3 nm spatial resolution “Figure 2”. HRTEM and CBED and precession diffraction coupled with JEMS simulations [2] are used to probe atomic structure order as well as to describe stress distribution. High resolution SEM was used to describe layer surfaces on a large 2 dimensional scale, providing information on thickness variations. When putting together the pieces of the puzzle brought by each technique, we show that we obtain quite a clear image of the alloy, thus providing valuable elements to the understanding of its optical properties. Results include and are not limited to stress induced composition variation around dislocations in agreement with theory, spiral growth composition fluctuation “Figure 2”, accurate description of pit dimensions and a better understanding of their origins “Figure 1”, interface disorder brought by dislocations, spiral growth induced thickness variation and an accurate description of defect creation and structural degradation with the increase of layer thickness. 1. 2.
J.-F. Carlin and M. Ilegems, Appl. Phys. Lett. 83, 668 (2003) P. A. Stadelmann, Ultramicroscopy Volume 21, Issue 2, 1987, Pages 131-145.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 79–80, DOI: 10.1007/978-3-540-85226-1_40, © Springer-Verlag Berlin Heidelberg 2008
80
Figure 1: Surface pits originating from screw component threading dislocations shown by weak beam dark-field thickness fringes
Figure 2: EDX Mapping showing periodic Indium peaks around a threading dislocation
Figure 3: HRTEM image of a mixed threading dislocation crossing a GaN/AlInN interface, along with the projected shear stress it is causing calculated by geometric phase analysis
81
TEM analyses of microstructure and composition of AlxGa1-xN/GaN distributed Bragg reflectors A. Pretorius, A. Rosenauer, T. Aschenbrenner, H. Dartsch, S. Figge, and D. Hommel Institute of Solid State Physics, University of Bremen, Otto-Hahn-Allee 1, 28359 Bremen, Germany
[email protected] Keywords: AlGaN/GaN DBRs, TEM, STEM, STEM-simulation
In this work we analyse the microstructure as well as layer thicknesses and Al concentration of AlxGa1-xN/GaN distributed Bragg reflectors (DBRs) by transmission electron microscopy. To gain a high reflectivity of the DBR, a high refractive index contrast Δn is necessary, i. e. high Al content x. On the other hand, this leads to built-in stress. Due to this, cracks and/or dislocations can form and thus the reflectivity can be reduced. An optimum stress compensation and the adjustment of the wavelength reflected by the DBR needs a precise control of the layer thicknesses and the Al content. The analysed DBR was grown by metal organic vapour phase epitaxy (MOVPE). About 1 µm AlGaN of an intended concentration x = 0.25 was deposited on top of (0001) oriented Al2O3. This was followed by 40 mirror pairs of GaN and AlGaN with intended concentration x = 0.45 and nominal thicknesses of 50 nm. Finally, a GaN cap layer was deposited. The concentrations of the AlGaN buffer and DBR layers were chosen in order to obtain an overall stress compensated structure. Cross-sectional TEM samples were prepared and analysed in a TITAN 80/300 equipped with an imaging CScorrector and operated at 300 kV. Optical microscopy and TEM exhibited very few cracks in the DBR (Figure 1). Scanning electron microscopy (SEM) analysis revealed that no cracks penetrated to the surface, i. e. all are overgrown. In addition, few voids were observed by TEM analysis inside the DBR. Evaluation of the layer thicknesses from STEM images reveals a slowly varying, approx. constant AlGaN layer thickness (Figure 2). In contrast, the GaN layer thickness varies significantly. Using high resolution STEM (HRSTEM, Figure 3) it was found that the GaN-AlGaN interfaces are comparably sharp (interface width ~2.2 nm), whereas the AlGaN-GaN interfaces are blurred (interface width ~6.5 nm). The Al concentration x of the DBR layers was also obtained from Z-contrast images. The image intensity I was simulated in dependence of x and TEM specimen thickness t using the STEMsim program [1]. For t exceeding 20 nm, the ratio IGaN/IAlGaN was found to be nearly independent of the actual value of t, i. e. only to depend on x. On basis of the simulated intensity ratio, the Al concentration was extracted from the measured Zcontrast images and is displayed in Figure 4. The derived concentrations of ~0.43 for the AlGaN DBR layers and ~0.21 for the AlGaN buffer layer are in very good agreement with concentration values obtained from X-ray diffraction (0.45 and 0.21, respectively).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 81–82, DOI: 10.1007/978-3-540-85226-1_41, © Springer-Verlag Berlin Heidelberg 2008
82
In summary, the investigated AlGaN/GaN DBR is of good structural quality. The Al concentrations of the buffer and DBR layers are very close to the intended values. Nevertheless, the GaN layer thicknesses vary considerably, which may reduce the reflectivity of the DBR. 1. 2.
A. Rosenauer, M. Schowalter, Springer Proceedings in Physics: Microscopy of Semiconducting Materials (MSM) conference 2007, Cambridge. Financial support by the Deutsche Forschungsgemeinschaft (DFG Grant no. FOR 506) is gratefully acknowledged.
Figure 1. Z-contrast image of an overgrown crack.
Figure 3. HRSTEM image showing a sharp interface between GaN-Al0 45Ga0 55N, but a blurred interface between Al0 45Ga0 55N-GaN.
Figure 2. DBR layer thicknesses as obtained from Z-contrast images.
Figure 4. Concentration profile of the DBR obtained from a Zcontrast image.
83
TEM study of quaternary InGaAsN/GaAs quantum well structures grown by molecular beam epitaxy T. Remmele1, M. Albrecht1, I. Häusler1, L. Geelhaar2, H. Riechert2, H. Abu-Farsakh3, and J. Neugebauer3 1. Institut für Kristallzüchtung, Max-Born-Str. 2, D-12489 Berlin, Germany 2. Qimonda (formerly Infineon Technologies Corporate Research Photonics), Otto-Hahn-Ring 6, D-81730 München, Germany 3. Max-Planck-Institut für Eisenforschung GmbH, Max-Planck-Straße 1, D-40237 Düsseldorf, Germany
[email protected] Keywords: InGaAsN, composition analysis, growth kinetics
In this study we report on the compositional analysis of quaternary InGaAsN/GaAs quantum well (QW) structures based on transmission electron microscope (TEM) investigations accompanied by theoretical ab-initio calculations. The pronounced band gap bowing by adding nitrogen to GaAs allows to reach the telecommunication wavelength range around 1.3–1.55 µm while staying lattice matched to the GaAs substrate by incorporating In. A sample series of InxGa1-xAs1-yNy with different nominal concentrations of In and N in the range of x = 0.1 – 0.4 and y = 0.01 – 0.05, respectively, were grown by radio-frequency plasma assisted molecular beam epitaxy and has been investigated by TEM. We used strain analysis of high-resolution TEM micrographs in combination with dark field imaging of the chemical sensitive (002)-reflection to evaluate the composition in the QW [1]. The evaluation of the dark field intensity depends on the scattering factors. For alloys the scattering factors are generally derived from atomic scattering factors using Vegard‘s rule. In recent publications [2,3] different scattering factors for InGaAs and GaAsN has been published. In these works the static atomic displacements [4] around individual In or N atoms, computed according to density functional theory, has been taken into account for the estimation of the scattering factors. However, in our evaluations we get a reasonable well correspondence between nominal and experimental values using scattering factors derived by Vegard‘s rule. The reason of this discrepancy is currently under investigation and will be reported. Figure 1 shows a dark field image of a GaAsN, an InGaAsN, and an InGaAs QW grown under identical conditions in one growth run. As shown in figure 2 we find at the bottom and also at the top interface of the InGaAsN QW a nitrogen enriched layer where the In concentration has its rising or trailing edge. The N-enriched layers occur in QW with an In concentration above x=0.2. The presence of these layers were also observed semi-quantitatively in energy filtered TEM measurements. On the ternary GaAsN QW no such enriched layers are present. The formation of the N-enriched layers is controlled by the surface kinetics during the growth. Ab-initio calculations show that while in bulk samples In-N pairs are
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 83–84, DOI: 10.1007/978-3-540-85226-1_42, © Springer-Verlag Berlin Heidelberg 2008
84
energetically preferable due to strain reduction, at the surface, where strain relaxation occurs, the chemical environment dominates the energetic relations. The result is a repulsive In-N interaction and a high kinetic barrier for N-diffusion to subsurface positions at the growth surface which lead to the observed In-N anti-correlation in InGaAsN quantum wells. 1. 2. 3. 4.
V. Grillo, M. Albrecht, T. Remmele, H. P. Strunk, A. Y. Egorov, and H. Riechert, Journal of Applied Physics 90 (2001), p. 3792. A. Rosenauer, M. Schowalter, F. Glas, and D. Lamoen. Physical Review B (Condensed Matter and Materials Physics), 72 (2005), p. 85326. K. Volz, O. Rubel, T. Torunski, S. D. Baranovskii, and W. Stolz, Appl. Phys. Lett. 88 (2006), p 81910. F. Glas, Physical Review B, 51 (1995), p. 825.
Figure 1. Dark field image with (002)-reflection of three quantum wells with different compositions (InGaAs, InGaAsN, GaAsN). The nominal concentrations of In and N in the quantum wells are x=0.39 and y=0.02, respectively.
Figure 2. Evaluated N-concentration (left) and In-concentration (right) of the quantum wells in figure 1. N-riche interface layers are observed for the quaternary InGaAsN QW.
85
Lattice polarity and capping of GaN dots studied by Z-contrast imaging J.L. Rouviere1, C. Bougerol2, J. Coraux2, B. Amstatt2 , E. Bellet-Amalric2 and B. Daudin2 CEA-Grenoble 17 rue des Martyrs 38054 Grenoble FRANCE 1. INAC/SP2M/LEMMA 2. CEA-CNRS group "Nanophysique et Semiconducteurs" jean-luc.rouviere@cea fr Keywords: nitride, quantum dot, polarity, STEM
In this work we show the interest of using Z-contrast images for analysing GaN quantum dots. Firstly it is shown that the polarity of GaN quantum dots can be determined by using a probe Cs-corrector. Secondly, the way GaN quantum dots are capped with AlN layers is analyzed. Samples were grown by Molecular Beam Epitaxy (MEB). GaN quantum dots were deposited on or embedded in AlN layers [1]. For the capping study, different thickness of AlN capping layers where deposited on GaN dots (Figure 2). Cross-sections were realised by mechanical polishing and ion milling. A FEI-TITAN microscope equipped with a CEOS probe Cs-corrector and working at 300kV was used for the Z-contrast images. The polarity of two kinds of GaN quantum dots has been determined : GaN dots grown on (0001) AlN surface (Figure 1) and GaN dots grown on (1100) AlN (not shown here). (0001) GaN have a symmetric shape whereas (1100) GaN dots tend to have an asymmetric shape because in our Ga-rich growh condition, growth is faster along [0001] than along [0001] [2]. Figure 1 outlines how the Ga-polarity has been determined, that is to say how the GaN bonds parallel to [0001] (or GaN bond vectors) are oriented with respect to the surface normal of the layers. In Figure 1f, N atomic columns are not visible as clear white spots, because the contrast of N columns (Z=7) is broad and faint compared to Ga column (Z=31). However the location of N columns can be determined by comparing the regions above and below the central Ga atoms, which is equivalent at looking the surroundings of positions N2 and N4. Tunnels positions are clearly determined. In Figure 2, Z-contrast images determine at once the shape of the AlN capping layer. For AlN capping layer having an equivalent thickness smaller than 4 monolayers (ML), AlN wet the GaN dots. For AlN thicknesses between 4 ML and 14 ML, AlN fills the gap between GaN layers. Above 14 ML, the surface of the AlN capping layer is again flat [1]. 1 2
J Coraux, B Amstatt, JA Budagoski, E Bellet-Amalric, JL Rouvière, V Favre-Nicolin, MG Proietti, H Renevier, B Daudin Phys. Rev. B 74 (2006) p. 195302 J.L. Rouvière, C. Bougerol, E. Bellet-Amalric, B. Amstatt, B. Daudin, submitted to APL
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 85–86, DOI: 10.1007/978-3-540-85226-1_43, © Springer-Verlag Berlin Heidelberg 2008
86
Figure 1 (a) High Resolution STEM image of a GaN at the surface of an AlN layer. (b) Atomic model of the wurtzite GaN projected on the (2,-1,-1,0) plane. In projection, two rectangular unit cells can be chosen. The left one is chosen in the other figures. (c) The left unit cell of a GaN crystal having a Ga-polarity orientation (surface normal is supposed to point upwards). (d) The left unit cell with a GaN crystal have a N-polarity orientation. (e) Image extracted from figure 1a). (f) Average of 10 images similar to figure 1e. N atomic column positions N1 and N2 (respectively N3 and N4) of a Gapolar crystal (respectively N-polar crystal) have been added to the picture. (g) Same image a figure 1f but with a slightly different contrast. The atomic structure of a Gapolar crystal has been added. Tunnels are clearly located. The difference between the regions above and below the central Ga atom of the rectangular cell is also clearly visible : the region below is darker than the region above, so the N-atomic column is situated above the central Ga atom.
Figure 2 Four Z-contrast images showing how AlN covers GaN dots for four different amounts of AlN : GaN material appears brighter than AlN. The numbers on the left of the picture give the number of equivalent AlN monolayers (ML) deposited on GaN dots. Above the AlN capping layer a thin GaN layer (2 ML) has been deposited in order to determine the shape of the AlN capping layer. On the top picture (4 ML) AlN wets GaN dots whereas on the bottom picture (14ML) AlN fills the gaps between GaN dots.
87
Investigation of swift ions damage in wide band gap wurtzite semiconductors S. Mansouri, I. Monnet, H. Lebius, G. Nouet and P. Ruterana CIMAP, UMR 6252 CNRS-ENSICAEN-CEA- UCBN, 6, Boulevard du Maréchal Juin, 14050 Caen Cedex pierre.ruterana@ensicaen fr Keywords: nitride semiconductors, AlN, GaN, InN, swift ions irradiation, ion tracks, band gap smearing, optical properties, TEM, nanodots, AFM
The wide band gap wurtzite semiconductors (AlN, GaN, InN) constitute an interesting family of materials with an extensive range of micro-electronic and optoelectronic applications. Moreover, they are close to ceramics, therefore fabricated devices are also due to operate in harsh environments (space, underwater, inside motors or nuclear reactors, …). As the data on the effect of irradiation by swift heavy ions is still scarce (GaN, AlN) or completely inexistent (InN), their behaviour in such an environment is not known or is still controversial. The case of AlN is particular since it also has been investigated in the form of polycrystalline material, starting at the time when it was only considered for the fabrication of ceramic based devices. In good quality monocrystalline material, only AlN, and GaN have started to be investigated. Indeed, most of the work has been carried out under ion bombardment at medium range energies (~100 keV) for which the contribution of the electronic energy loss processes is rather negligible in the formation of defects. In the high energy range, wurtzite GaN layers were irradiated at 300K with 200 MeV 197Au16+ (Se = 34 keV/nm) and tracks were identified by TEM with a diameter of about 10nm. They were characterized by a structural disordering but no amorphous phase formation was reported [1]. More recently, damage accumulation was analyzed with 230 MeV Pb27+ at room temperature and at 513K. From RBS spectra, it was deduced that rapid damage accumulation and efficient erosion occur at a rather low value of the electronic energy deposition [2]. We can also quote irradiations with 150 MeV Ag12+ [3] and 100 MeV Ag8+ and O7+[4]. Probably due to the lack of good quality material, InN has not yet been studied and no report on the material behaviour under high energy ions is yet available. Therefore, it is of fundamental interest to carry out a systematic analysis of the electronic excitation in the energy deposition processes into these high expectation materials. Our investigations carried out with Xe (22.5 keV/nm) under grazing incidence show the formation of arrays of nanodots by single ions (Figure 1a). Moreover, a number of experiments have been also carried out with Pb ion beam on TEM thin foils, the first results indicate that there is a difference between AlN, GaN. No tracks were observed in AlN, whereas nanometer crystalline tracks are formed in GaN (Figure 1b).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 87–88, DOI: 10.1007/978-3-540-85226-1_44, © Springer-Verlag Berlin Heidelberg 2008
88
The evolution of the optical properties versus the ion fluence has also been investigated, for GaN, it has been found that, as the ion dose is increased above 10exp13 at*cm-2, the band gap is rapidly smeared out due to defects accumulation.
Figure 1 : a) arrays of nanodots in GaN irradiated at 1° xith Xe 0,7Me/u; b) Small tracks in GaN 0,5 MeV/u Pb 1. 2. 3. 4.
S.O. Kucheyev, H. Timmers, J. Zou, J.S. Williams, J. Jacadish and G. Li, J. Appl. Phys. 95, (2004)5360 C.H. Zang, Y. Song, Y.M. Sun, H. Chen, Y.T. Yang, L.H. Zhou and Y.F. Jin, Nucl. Instr. and Meth.B, 256, (2007)199 N. Sathish, Nucl. Instr. and Meth.B, 256, (2007)281 V. Suresh Kumar, Nucl. Instr. and Meth.B, 244, (2007)145
89
A TEM analysis of the damage formation in thin GaN and AlN layers during rare earth ion implantation at medium range energy F. Gloux, M.P Chauvat and P. Ruterana CIMAP, UMR 6252, CNRS-ENSICAEN-CEA-UCBN, 6, Boulevard Maréchal Juin, 14050 Caen, France pierre.ruterana@ensicaen fr Keywords: GaN, ion implantation, nanocrystallisation, basal stacking faults, prismatic stacking faults, rare earth doping, TEM
Rare earth (RE) doped GaN has been the subject of research over the past few years due to promising light emission applications [1]. In optoelectronics, particularly, interesting results have been recently obtained, for instance laser action at room temperature (RT) have been reported in Eu doped GaN [2]. These applications were achieved using GaN layers doped in situ by molecular beam epitaxy. Ion implantation as a doping technique has interesting advantages, i.e. control of the doped area and easy lateral integration. However it causes a large amount of structural defects in the implanted layers. As the GaN fusion temperature is very high, post-implant annealing performed for RE activation should be carried out well above 1000°C. During the last few years, a renewed interest has been shown in understanding the structural damage build-up in the implanted GaN by a number of recent reports [4-5]. Recently, an improved optical activation of REs was obtained for annealing temperatures as high as 1300°C [3] using an AlN capping. It has been shown that the 'amorphous layer' that usually forms inside the implanted layer at high fluences was reported to be instead made of broken crystals [6]. These results demonstrate that the knowledge of the implantation damage build-up in GaN has not yet been completed. In this work, the nature of the damage in GaN implanted by rare earth ions at 300keV and room temperature has been investigated by transmission electron microscopy versus the fluence, from 7x1013 to 2x1016at/cm2, using Er, Eu or Tm ions implantation. The density of point defect clusters has been found to increase with the fluence. In GaN, from about 3x1015at/cm2, a highly disordered 'nanocrystalline layer' (NL) starts to form at the GaN surface. Its structure exhibits a mixture of voids and misoriented nanocrystallites (Figure 1). Basal stacking faults (BSFs) of I1, E and I2 types have been observed from the lowest fluence, they are I1 in majority. Their density increases and saturates when the NL appears. Many prismatic stacking faults (PSFs) with Drum atomic configuration have been observed [7, 8]. The I1 BSFs are shown to propagate easily through GaN by folding from basal to prismatic planes thanks to the PSFs (Figure 2: position of the PSF indicated by arrow). When implanting through a 10nm AlN cap, the NL formation threshold goes up to about 3x1016at/cm2, which support the point that the AlN cap plays a protective role against the damage formation
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 89–90, DOI: 10.1007/978-3-540-85226-1_45, © Springer-Verlag Berlin Heidelberg 2008
90
in GaN up to the highest fluences [3]. The flat surface after implantation and the absence of SFs in the AlN cap indicate also the high resistance to the damage formation. 1. 2. 3. 4. 5. 6. 7. 8.
D. S. Lee and A. J. Steckl, Appl. Phys. Lett. 80, (2002)1888 J. H. Park and A.J. Steckl, Appl. Phys. Lett. 85, (20044588 Lorenz, U. Wahl, E. Alves, S. Dalmasso, R. W. Martin, K. P. O’Donnell, S. Ruffenach and O. Briot, Appl. Phys. Lett. 85, (2004)2712 C. Liu, B. Mensching, M. Zitler, K. Volz and B. Rauschenbach, Phys. Rev. B 57, (1998)2530 S. O. Kucheyev, J. S. Williams, C. Jagadish, J. Zou and G. Li, Phys. Rev. B 62, (2000)7510 F-R. Ding, W-H. He, A. Vantomme, Q. Zhao, B. Pipeleers, K. Jacobs, I. Moerman , Materials Science in Semiconductor Processing 5, (2003) 511 P. Vermaut, P. Ruterana and G. Nouet, Appl. Phys. Lett. 74, (1999) 694 F. Gloux, T. Wojtowicz, P. Ruterana, K. Lorenz, and E. Alves, J. Appl. Phys. 100, (2006)073520
Figure 1: a)Nanocrystalline layer with voids (arrow) in the surface area of a GaN subsequent to 4*e1015 at/cm2 Eu implantation at 300 KV. b)The corresponding TFF
1 nm Figure 2: An I1 basal stacking fault which folds to and from the prismatic plane, the positions of the stacking fault segments have been marked, see the cubic stackings.
91
Characterization and modelling of semiconductor quantum nanostructures grown by droplet epitaxy D.L. Sales1, J.C. Hernandez2, P.A. Midgley2, A.M. Beltran1, A.M. Sanchez1, T. Ben1, P. Alonso-González3, Y. Gonzalez3, L. Gonzalez3 and S.I. Molina1 1. Departamento de Ciencia de los Materiales e I. M. y Q. I., Universidad de Cadiz, Campus Univ. Rio San Pedro, 11510 Puerto Real, Spain 2. Department of Materials Science and Metallurgy, University of Cambridge, Pembroke Street, Cambridge, CB2 3QZ, UK 3. Instituto de Microelectronica de Madrid (IMM-CNM, CSIC), Isaac Newton, 28760 Tres Cantos, Spain
[email protected] Keywords: quantum dots, quantum rings, electron tomography.
One of the main requirements for the development of quantum computing is the ability of manufacturing single photon emitters. Self assembled semiconductor nanostructures are ones of the most reliable candidates for this application, once control of size and spatial location is achieved. The droplet epitaxy technique allows growth of low density distributions of nanostructures with good optical quality, constituting a promising method for single photon devices and quantum applications [1]. In this work two samples have been analysed: (i) InAs quantum dots (QDs) nucleated on GaAs nanoholes that were formed by the crystallization of Ga droplets under As atmosphere [1], and (ii) GaSb quantum rings (QRs) formed by the crystallization of Ga droplets under Sb atmosphere. In this case, surface QR were also grown after growth of a 20 nm thick GaAs cap layer. In both cases, after the capping growth process, it was observed the formation of surface GaAs mounds that, as shown in this work, would be related to the location of the buried nanostructures. The capacity of transmission electron microscopy (TEM) to extract fine-scale information about the internal structure has been essential to understand the growth of these devices. Conventional TEM allows the characterization of structural defects which can appear during the capping of the nanostructures reducing the photoluminescence emission. It is observed in CTEM images that every buried mound is correlated with a mound on surface (see Figure 1). This fact enables the density of buried nanostructures to measured, directly related to the number of emitters, by analysing the sample surface. Three-dimensional scanning transmission electron microscopy (STEM) has been used to characterize GaSb QRs grown on a GaAs mounds. Reconstructed STEM tomograms show contrast arising from structural defects. These defects (probably dislocations) run from the buried mound to the surface mound. The 3D reconstruction (Figure 2) allows a detailed characterization of the structure, including the shape and size of the QR structure and nanohole, and the spatial shift between the buried and the superficial QR.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 91–92, DOI: 10.1007/978-3-540-85226-1_46, © Springer-Verlag Berlin Heidelberg 2008
92
Additionally, the strain state of the structures has been calculated from elasticity theory using finite element analysis. The places where the nanostructures nucleate correspond with those with larger in-plane lattice parameter, i.e. lower elastic energy. 1. 2.
P. Alonso-Gonzalez, B. Alen, D. Fuster, Y. Gonzalez and L. Gonzalez, Appl. Phys. Lett. 91 (2007) 163104. This work has been supported by MEC (TEC2005-05781-C03-01 and 02/MIC), SANDiE and ESTEEM European networks (Contracts NMP4-CT-2004-500101 and 026019 ESTEEM), and Junta de Andalucía (PAI research group TEP-120).
Figure 1. CTEM image of a sample where InAs QDs have been grown on GaAs mounds. Two buried mounds are shown correlated with ones on the surface.
Figure 2. Surface render of a STEM tomographic reconstruction of a GaSb QR grown on a GaAs mound to reveal the complex shape of the QR and a nanohole.
93
Transmission Electron Microscopy Investigation of Self-Organized InN Nano-columns H. Schuhmann1, C. Denker1, T. Niermann2, J. Malindretos1, A. Rizzi1, M. Seibt1 1. IV. Physikalisches Institut, Georg-August-Universität Göttingen, D-37077 Göttingen, Germany 2. now at: Institut für Optik und Atomare Physik, Technische Universität Berlin, D-10623 Berlin, Germany
[email protected] Keywords: InN, nano-columns, wires
Semiconductor InN nano-columns have electronic properties which make them a promising candidate for novel photovoltaic devices. Molecular-Beam Epitaxy (MBE) grown InN on p-Si(111) substrates forms selforganized InN nano-columns under suitable conditions [1]. In a bimodal growth regime nano-columns with lengths of up to 2 microns and diameters down to 20 nm were observed. Because the shape of the nano-columns sensitively depends on growth parameters their crystal quality and characteristics were studied by Transmission Electron Microscopy (TEM). High-resolution TEM of a cross-section specimen at the interface between the crystalline InN nano-columns with a growth direction along the [0001] direction and the silicon substrate indicates the existence of an amorphous surface layer with a thickness of about 2nm. Additionally, a predicted tilt [2] between the nano-columns and the silicon substrate of about 23 degrees was observed. In order to study the crystal quality of the InN nano-columns along the rod axis projection, Focused Ion Beam (FIB) was used to prepare a TEM sample from an individual, specially selected long nanocolumn obtained from the bimodal growth regime. High-Resolution TEM micrograph (see Figure 1) of this slice showed a high crystal quality with no defects or oxidation. In particluar, no sub-surface microstructure or chemistry has been observed indicating homogeneous InN nano-columns. In order to analyse a possible distribution of axial rotations of the columns against the silicon substrate it is necessary to study a large ensemble of nano-columns along the growth direction. This is carried out by a bevel-view specimen preparation. Here a TEM lamella was cut out by an angle of 10° to the interface by the FIB (see Figure 2). As is seen in Figure 3 it is additionally possible to study the development of the number and diameter of the nano-columns with the distance to the silicon interface. 1. 2.
Christian Denker, Joerg Mailindretos, Florian Werner, Friederich Limbach, Henning Schuhmann, Michael Seibt, Angela Rizzi, Self organized growth of InN-nanocloumns on pSi(111) by MBE, physica status solidi, accepted (2008) Christian Denker, Diploma thesis, Universität Göttingen (2007)
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 93–94, DOI: 10.1007/978-3-540-85226-1_47, © Springer-Verlag Berlin Heidelberg 2008
94
Figure 1. HRTEM micrograph of a single InN nano-column prepared by focussed ion-beam technique. The crosssection is parallel to the [0001] growth direction of the nanocolumns.
Figure 2. Sketch of a bevel-view sample preparation using focused ion beam
Figure 3. TEM micrograph of the bevel-view specimen. The silicon substrate can be seen in the lower left corner.
95
Investigations on a dilute magnetic semicondutor (Ga1-xMnxAs) by conventional TEM and EELS M. Soda1, U. Wurstbauer, M. Hirmer, W. Wegscheider, J. Zweck 1. University of Regensburg, Institute of Experimental and Applied Physics, Universitätstrasse 31, 93040 Regensburg, Germany
[email protected] Keywords: GaMnAs, EELS
The Dilute Magnetic Semiconductor (DMS) Ga1-xMnxAs offers good prospects for the integration of ferromagnetic and semiconducting properties for use in future “spintronic” applications [1]. GaMnAs is grown under low temperature conditions, leading to the incorporation of various defects. The location and type of these defects determines the Curie temperature (Tc). Low temperature annealing generally increase Tc, while annealing at higher temperatures leads to a decrease of Tc [2, 3]. Therefore it is important to investigate the structure of GaMnAs in various states of annealing. The investigated samples consists of 20-80 nm thick Ga1-xMnxAs layer grown by Molecular Beam Epitaxy (MBE) with x varying between 1% and 6%. As grown and annealed materials were compared. From 002 DF images (see Figure 1) a homogeneous doping with Mn can be proven. In the annealed one, as expected, an about 2 nm thick Mn-oxide layer at the surface is present (see Figure 2). Its composition was investigated by EELS, clearly indicating an oxygen and a Mn peak. It is known that the temperature treatment leads to a diffusion of Mn to the surface [4]. The composition of the thin dark strip (see arrow in Figure 2) on the top of the GaMnAs layer remain unidentified. An excessive annealing (68h @ 230°C) on a sample was performed and the results are shown in Figure 3. In addition to the Mn-oxide layer and the dark strip, clusters are formed in about 8 nm deep cavities. So far it has not been possible to determine the composition or the lattice constant of the clusters due to their instability under the beam. Cooling the specimen at liquid nitrogen temperature is expected to help. For a concise interpretation of the results one has to bear in mind that during the ion milling the specimen suffers an increase in temperature. This increase may reasonably be assumed to be comparable to the annealing temperature (180- 250 °C), thus leading to a preparation artifact.
1. 2. 3. 4.
Y. Ohno et al, Nature 402 (1999), 790. S. J. Potashnik et al, App. Phy. Let. 79 (2001). J. Sadowski, Mat. Sci.-Poland 24 (2006). K. W. Edmonds et al, Phys. Rev. Let. 92 (2004), 037201
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 95–96, DOI: 10.1007/978-3-540-85226-1_48, © Springer-Verlag Berlin Heidelberg 2008
96
a)
20 nm
b)
20 nm
Figure 1. 002 DF images show a homogeneous doped layer. a) as grown b) annealed.
a)
10 nm
Oxygen
Manganese
532 eV
640 eV
b)
5 nm
Figure 2. a) as grown sample, b) annealed sample with about 2 nm Mn-oxide layer, inset) EELS spectrum of the Mn-oxide layer.
20 nm
Figure 3. Micrograph of an excessive annealed Specimen. It can be seen a Mn-oxide layer of about 10 nm at the surface of the sample and cluster in 10 nm deep cavitys.
97
About the determination of optical properties using fast electrons M. Stöger-Pollach University Service Center for Transmission Electron Microscopy, Technische Universität Wien, Wiedner Hauptstrasse 8-10, A-1040 Wien, Austria
[email protected] Keywords: optical properties, EELS, retardation
In the last years spatial and energy resolution of transmission electron microscopes (TEM) were improved tremendously by the invention of Cs-correctors and monochromators. Using electron energy loss spectrometry (EELS) in such TEMs makes the determination of optical properties of semiconductors accessible even for layers thinner than the wave length of light, where optical methods fail. It was long a time thought that simply using the Kramers-Kronig relations can give accurate information on the dielectric function and all the other optical constants. Frequently discrepancies between optical methods and EELS were found. The reason for this are retardation effects and Čerenkov radiation [1], emitted as soon as the speed of the probe electrons v is faster than the speed of light inside the sample c/n – with n as the refractive index: v>c/n. (1) If the problem of the zero loss peak (ZLP) removal is solved properly [2], there are a few possibilities to increase the accuracy of the determination of optical properties with fast electrons: (a) in the frame work of Kröger’s theory an iterative routine can be set up removing the relativistic effects off-line. (b) a reduction of the incident beam energy would change the unequal sign in Eq. (1) depending on the materials refractive index n. (c) an experimental difference method [3] can be set up subtracting the relativistic energy losses, which have an extremely narrow angular distribution. For the experimental demonstration we chose SiNx:H, because it shows slight relativistic effects for a 200 keV electron beam (v>c/n) but for 60 keV the speed of the electrons don’t exceed the speed of light inside the sample. Figure 1 demonstrates the ZLP removal problem for (left) an experiment with v
c/n on SiNx:H using several ZLP removal routines. It is found, that even if a correct band gap value is determined (by the power law fit method) the resulting data cannot be used for Kramers-Kronig Analysis (KKA). In Figure 2 we demonstrate the precision of the iterative routine removing relativistic effects by comparison with an experiment with v
E. Kröger, Zeitschrift für Physik 216 (1968) 115 – 135 M. Stöger-Pollach et al., Ultramicroscopy 107 (2007) 1178 – 1185 M. Stöger-Pollach, Micron doi:10.1016/j micron.2008.01.23
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 97–98, DOI: 10.1007/978-3-540-85226-1_49, © Springer-Verlag Berlin Heidelberg 2008
98
Figure 1: Comparison of ZLP removal routines for 60 keV (left) and 200 keV (right) experiments on 0.34 λ thick SiNx:H samples.
Figure 2: Experimental prove of the accuracy of an off-line correction based on Kröger’s theory. Left: Experiment performed with 60 keV avoiding retardation losses and right: experiment performed with 200 keV electrons and removing retardation losses off-line. Finally on both spectra KKA was performed in order to calculate the refractive indices of the two layers Figure 3: Calculation from 0-0.125 mrad showing that the surface intensities and the Cerenkov contributions can be excluded from the VEELS spectrum, if these small q-values can be excluded from the recording of the VEELS spectrum. Left: GaP using 60 keV, Right: GaP using 200 keV beam energy. B: Sketch of the principle experimental setup (From [2]). The Hochschuljubiläumsstiftung der Stadt Wien, contract Nbr. H-01585/2007, is kindly acknowledged for funding.
99
Mapping uncompensated spins in exchange-biased systems by high resolution and quantitative magnetic force microscopy H. J. Hug, M. Marioni, S. Romer, I. Schmid and S. Romer Empa, Überlandstrasse 129, CH-8600 Dübendorf, Switzerland hans-josef [email protected] Keywords: magnetic force microscopy, exchange bias effect, uncompensated spins
Magnetic Force Microscopy is an ideal tool to image magnetic stray fields emanating from surfaces but also from hidden interfaces of magnetic samples. A lateral resolution of 10nm is routinely obtained on flat samples. Tip calibration techniques were developed for a quantitative evaluation of the magnetic surface charge or surface dipole density from the measured MFM signal [1,2]. The origin of the exchange bias (EB) effect has been traced back to the existence of pinned uncompensated spins (UCS) in the antiferromagnet (AFM) or at its interface. However, the understanding of the underlying mechanism is still clouded by contradictory reports: Ohldag et al. [3] used XMCD to extract the direction and density of pinned UCS from the vertical shift of element specific magnetization loops. In their interpretation, the positive vertical shifts found for all investigated EB materials reflects a parallel coupling of the UCS to the spins of the ferromagnet (FM). Tsunoda et al. [4] used a similar experimental method but did not find any vertical shift in similar EB materials, although these materials showed a large EB-effect. Furthermore, Kappenberger et al. [5] (magnetic force microscopy) and Eimüller et al. [6] (XMCD PEEM) reported an antiferromagnetic coupling between the UCS and the FM spins. In order to clarify the role of the UCS for the EB-effect different perpendicular exchange-biased AFM/FM multilayers were prepared by magnetron sputtering. The FM layers consisted of CoPt and CoPd multilayers exhibiting a strong perpendicular magnetic anisotropy. For the AFM layers either CoO or MnIr was used. Magnetometry and magnetic force microscopy measurements were used advantageously to demonstrate the co-existence of pinned UCS that are parallel and antiparallel to the cooling field in metallic (IrMn) and oxidic (CoO) EB systems. We found that the exchange-bias-effect (EB-effect) is a result of pinned interfacial UCS, which are antiparallel to the spins of the ferromagnet. The often observed positive vertical shift of the magnetization loop after field cooling is due to pinned UCS that align parallel to the cooling field, but are of little importance for the EB-effect [7]. Given that most experimental techniques (including those used in our work [5,7]) measure the sum of both spin groups indiscriminately, contradictory results can arise. Our work may provide guidelines for the design of experiments that can correctly determine the densities of those UCS that do contribute to the EB effect. In further experiments, the distribution of density of the UCS was imaged on the length scales of single grains. A surprisingly strong fluctuation of the local UCS density
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 99–100, DOI: 10.1007/978-3-540-85226-1_50, © Springer-Verlag Berlin Heidelberg 2008
100
(UCSD) was observed. A correlation between the UCSD and the local exchange field was performed. Clearly, a high UCSD results in a high local exchange bias field. Regions with an anti-biasing effect were found. Using grain-boundary engineering, exchange-biased materials without such regions could be fabricated that showed a substantially increased exchange bias effect. 1. 2. 3. 4. 5. 6. 7.
P. J. A. van Schendel, H. J. Hug, B. Stiefel, S. Martin, H.-J. Güntherodt, J. Appl. Phys. 88 (2000), p435 M. A. Marioni, N. Pilet, A.V. Asworth, R. C. O'Handley, H. J. Hug, Phys. Rev. Lett. 97 (2006), p027201 H. Ohldag et al., Phys. Rev. Lett., 87 (2001), p247201. M. Tsunoda et al., Appl. Phys. Lett. 89 (2006), 172501 P. Kappenberger, S. Martin, Y. Pellmont, H.J. Hug, J.B. Kortright, O. Hellwig, and E.E. Fullerton, Phys. Rev. Lett. 91 (2003), p267202 T. Eimueller et al., J. Appl. Phys. 85 (2004), p2310. I. Schmid, P. Kappenberger, O. Hellwig, M. Carrey, Eric E. Fullerton, H. J. Hug, Euro Phys. Lett. 81 (2006), p17001
Figure 1. MFM images of a CoO/CoPt-multilayer antiferromagnet/ferromagnet sample. Panels a) shows the domains of ferromagnetic CoPt-multilayer after zero-field cooling and after a field of 100mT (panel b) and 200mT (panel c) is applied. Saturation of the ferromagnetic layer is obtained at 300mT (panel d and e). Then, the pinned uncompensated spins at the antiferromagnet/ferromagnet interface become visible (panels d and e). The yellow lines visible in panels d) and e) are guides for the eye to indicate the walls of the ferromagnetic domain states after zero-field cooling and at 200mT.
101
Ferroelectric materials and structures suitable for data storage: The role of microscopies in establishing preparation-microstructure-property relations D. Hesse1, M. Alexe1, K. Boldyreva1, H. Han1,2, W. Lee1, A. Lotnyk1, B.J. Rodriguez1, S. Senz1, I. Vrejoiu1, and N.D. Zakharov1 1. Max Planck Inst. of Microstructure Physics, Weinberg 2, D-06120 Halle, Germany 2. Dept. of Mater. Sci. and Eng., Pohang University of Science and Technology, Korea [email protected] Keywords: ferroelectrics, superlattices, nanostructures, microscopies
Among the various possible routes towards solid-state non-volatile random access memories (NV-RAMs) of high memory density, ferroelectric random access memories (FRAMs) offer very good prospects. Non-volatility is provided by the ionic character of the signal, and switching by an electric field is sufficiently fast and free from crosstalk. In view of these excellent prospects, ultrathin epitaxial films, multilayers, superlattices, and nanostructure arrays made from (anti-)ferroelectric perovskite or perovskitelike oxides as PbZrO3 (PZO), Pb(Zr,Ti)O3 (PZT) or (Bi,La)4Ti3O12 (BLT) are a most actual subject of research in materials science. Modification and tuning of interesting properties is possible by defect and orientation engineering in thin films, by variation of composition, layer thickness, strain or crystallographic orientation in multilayers and superlattices, and by choosing lateral size, pitch or crystallographic orientation of nanostructure arrays. Preparation by pulsed laser deposition (PLD) offers a number of advantages, especially in research. Ultrathin epitaxial films or strained superlattices (Figure 1), but also well-ordered, large-area arrays of ferroelectric nanostructures and nanocapacitors (Figure 2) can conveniently be prepared by PLD. The deposition of nanostructure and nanocapacitor arrays requires the application of appropriate nanoscale deposition masks made from metallic or well-ordered anodic alumina (AAO) layers. One of the main advantages of PLD is the possibility to extensively vary the deposition conditions in order to establish preparation-microstructure-property relations. Such relations can be studied in detail, comprising, e.g., the structure of 90° and 180° ferroelectric domain boundaries (e.g., [1]) and their role in switching processes (e.g., [2]). As will be shown, microscopies like AFM, SEM, piezoresponse-mode AFM (PFM), and (high-resolution) TEM are significant tools to study these relations. Plan-view and cross sectional (high-resolution) TEM images, as well as SEM and AFM topography images are used to characterize the microstructure of the substrates and the grown superlattices and nanocapacitor arrays (Figures 1,2), whereas PFM (Figure 2) and its recently developed switching-spectroscopy variant (SS-PFM) [2] are applied in studies of the local switching properties and domain dynamics. 1. 2.
C.-L. Jia, S.-B. Mi, K. Urban, I. Vrejoiu, M. Alexe, D. Hesse, Nat. Mat. 7 (2008) 57. S. Jesse, B.J. Rodriguez, S. Choudhury, A.P. Baddorf, I. Vrejoiu, D. Hesse, M. Alexe, M.A. Eliseev, A.N. Morozovska et al., Nat. Mat. 7 (2008) 209.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 101–102, DOI: 10.1007/978-3-540-85226-1_51, © Springer-Verlag Berlin Heidelberg 2008
102
Figure 1. (a,b) AFM topography images (3 x 3 μm2) of (a) a SrTiO3 (100) substrate with 0.1° miscut, and (b) a PZO/PZT(80/20) superlattice (overall thickness 100 nm; layer thickness 12.5 nm). (c,d) TEM cross section images of a coherently strained PZO/PZT(80/20) superlattice (overall thickness 150 nm; layer thickness 8 nm) on a PZT(20/80) buffer layer and a SrRuO3 electrode on a vicinal SrTiO3 substrate.
Figure 2. (a) SEM image of an as-prepared PZT nanoisland array with part of the ultrathin AAO mask. (b) TEM cross section image of a regular Pt/PZT/Pt nanocapacitor array. (c)-(f) AFM/PFM images (260 x 260 nm2) of a Pt/PZT/Pt nanocapacitor array: (c) topography; (d)-(f) piezoresponse, viz. (d) before switching, (e) after positive switching of two capacitors applying +3V, and (f) after negative switching of one of the two previously switched capacitors applying -3V.
103
Electronic structures at Magnetic Tunnel Junction interfaces: EELS experiments and FEFF calculations K. March, D. Imhoff, G. Krill, C. Colliex Lab. Physique des Solides, UMR CNRS-Université Paris XI, 91405 Orsay, France [email protected] fr Keywords: Heterostructures, spintronic, EELS, multiple scattering calculation
Electron transfer between the electrodes in a Magnetic Tunnel Junction (MTJ) is spin-dependent and directly related to the relative orientation of the magnetization of the two ferromagnetic layers on each side of the insulator barrier. TMR (tunnel magnetoresistance) values of several hundreds of % have been measured for the present MTJ generation, however well below the theoretical expectations. Higher TMR values measured on the epitaxial Co(Fe)/MgO/Co(Fe) system, reflect the position of the Fermi level which lies in the d-band where the electrons with Δ5 symmetry are only partly spin-polarized. Bridging experimental results with theoretical modelling requires a deeper investigation of the hybridization with the d electrons of transition atoms at the interfaces. In-situ XPS measurements on the Fe/MgO [1] have revealed that the hybridization between the Fe(d) and O(p) electrons seems to be rather small. However, we have no information about the CoFe/MgO system except a recent work (CoFeB [2]). We have therefore addressed this issue by recording EELS spectra of the O-K edge at sub-nanoscale range and by simulating the fine structures with multiple scattering calculations (FEFF 8.4). Co0 6Fe0 4/MgO/Co0 6Fe0 4 epitaxial samples on MgO substrates have been grown by Molecular Beam Epitaxy (MBE) at LPM Nancy. The atomic structure of the interfaces has been checked by HRTEM observations on a FEG-TEM equipped with a Cs corrector at CEMES Toulouse. EELS experiments resolved both spatially (< 0.6 nm) and energetically (< 0.5 eV) have been performed with a STEM microscope at LPS-Paris-Sud Orsay (3D spectrum-image 128*128*1340 pixels or less, core-loss area study (elemental profiles, ELNES extraction, branching ratio,…). O K-edges, directly extracted from spectrum-images (Figure 1A), show that O2p and (Fe,Co)3d bonding (oxidized TM) as well as e-beam induced O2 desorption, manifest themselves by the appearance of pre-edge structures located between 528 and 535 eV. FEFF calculations of the O K-edge spectra in the last interface plane of MgO confirm the appearance of prepeak structures depending on the Co(or Fe) atom position (Figure 2). They also show that only a slight longitudinal shift of the bcc transition metal structure relative to the MgO one, may produce a noticeable modification of the preedge on a simple “perfect” TM-O interface. This is of prime importance to understand the origin of the high TMR reported in this system. Experimental O K-edges (Figure 1B extracted from “line” or “sum” spectra) exhibit very similar “shapes” at the “top” and “ bottom” interfaces, with weak features in the prepeak region more similar to the hollow than to the apex calculated profiles, in agreement with the published XPS data [2]. These first results will be further developed for improving our understanding of the electronic properties of MTJ interfaces and effects on transport properties.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 103–104, DOI: 10.1007/978-3-540-85226-1_52, © Springer-Verlag Berlin Heidelberg 2008
104 1. 2. 3. 4.
S. Yuasa et al, Appl. Phys. Lett. 89 (2006), p 042505. J.J. Cha et al., Appl. Phys. Letters 91 (2007), p 062516 N. Bonnet, N. Brun, C. Colliex, Ultramicroscopy 77 (1999), p 97 Thanks are due to S. Andrieu and colleagues at LPM Nancy for specimen elaboration, to E. Snoeck and V. Serin at CEMES, Toulouse for collaboration. K.M. acknowledges ALTIS for her CIFRE thesis grant. The EC programme ESTEEM is also acknowledged for its support.
Figure 1. Experimental EELS results for the O K-edge. (A) reference data (≤ 0.2eV/ch): (i) pure MgO substrate, (ii) irradiation damage in MgO (chronospectroscopy (50 x 2 s)), (iii) oxided FexCo(1-x). (B) (upper part) as-acquired line scan across the MgO/FeCo heterostructure (0.2 eV/ch) and (lower part) sum of 128 spectra along few decades of nm at different spatial beam positions (“bottom” and “top” interfaces, “center” of the barrier), (0.3 eV/ch).
Figure 2. (A) Different positions of Co(or Fe) atom are considered relative to the central O atom in the last plane of the MgO structure: in “apex” or in the “hollow” site position. (B) Corresponding theoretical O K-edges calculated using FEFF 8.4 (with 500 at.): (i), (ii) (“apex” position) and (iii) (“hollow” site). Spectra (ii) and (iii) were convoluted by a 1eV Gaussian (FWHM)) in order to take into account of experimental conditions.
105
Stability and reaction of magnetic sensor materials studied by atom probe tomography G. Schmitz1, C. Ene2, H. Galinski1, V. Vovk1 1. Institut für Materialphysik, Westf. Wilhelms-Universität, Wilhelm-Klemm-Str. 10, 48149 Münster, Germany 2. Institut für Materialphysik, Universität Göttingen, Friedrich-Hundt-Platz 1, 37077 Göttingen, Germany [email protected] Keywords: GMR sensors, atom probe tomography, thermal reaction, Cahn-Hilliard-theory
State-of-the-art magnetic sensors usually consist of thin film multilayers with a periodicity of a few nanometers only. The significant contribution of interfaces and grain boundaries makes these nano-scaled materials inherently unstable and, even more puzzling, their high density of defects may accelerate atomic transport in an unpredictable way. Induced by the nanocrystalline microstructure of the sputtered thin films, reactions develop on a complex morphology which requires three-dimensional high resolution analysis as it is provided by atom probe tomography in a unique way. In the talk we will address the reaction of Cu/Py (Py stands for the soft magnetic Ni81Fe19 alloy) and of the Cu/Co model system. Compared to the frequently used Cu/Co sensors, multilayers of Cu/Py are distinguished by very low hysteresis which is of advantage for the design of position or orientation sensors. On the other hand, the thermal stability of these layer systems is rather low. What are the dominant structural mechanisms of thermal degeneration? We sputter-deposited thin film multilayers on top of tungsten substrate tips and studied the chemical structure after isochronal heat treatments in a temperature range from 150°C to 500°C [1]. Since the deposited layers reveal a columnar, nanocrystalline structure, one may expect that the dominant transport proceeds by grain boundary diffusion. Indeed, transport along grain boundaries is demonstrated by segregation zones in the tomographic volume reconstructions (see Figure 1a). In particular, grain boundaries inside Py appear enriched in Cu to surprisingly high amounts, up to 54at%. Such a Cu content would be way enough to insulate individual Py grains magnetically. However, these segregation zones develop only at temperatures higher than 350°C. In consequence, grain boundary transport cannot be made responsible for GMR degeneration starting already at much lower temperature. Due to the outstanding resolution of atom probe tomography, it is possible to detect even minor chemical modifications at the Cu/Py layer interface. So, we could observe in our experiments that the Cu concentration gradient at the interfaces decreases from about 1.5 nm-1 to about 1.0 nm-1 during 20 min annealing at 250°C due to a short-ranged volume diffusion. Such a modification seems to be negligible. However, in view of the typical single layer thickness of about 2 nm, it means that a considerable fraction of the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 105–106, DOI: 10.1007/978-3-540-85226-1_53, © Springer-Verlag Berlin Heidelberg 2008
106
volume has become already intermixed and in consequence the GMR amplitude has decreased significantly. Volume diffusion between insoluble metallic layers is quite surprising. In order to identify the physical basis of this process, we performed similar experiments with other model systems and found this short-ranged diffusion as a general behavior. This allows the conclusion that the mixing depth at the interface, although temperature dependent, must be controlled by a non-diffusive mechanism. Indeed, it is possible to describe the measured temperature dependence of the interface width by a Cahn-Hilliard ansatz (see Figure 1b), which predicts a maximum limit of the concentration gradient. So, as our main conclusion, we state that the thermal degeneration of the GMR amplitude is controlled by the concentration gradient term in the Gibbs energy. With atom probe tomography it is possible to prove this mechanism even on a length scale below one nanometer. C. Ene et al., Acta Mater. 5 (2005) 3383. P. Stender, C. B. Ene, H. Galinski, G. Schmitz, Intern. J. Mat. Res. (in press)
Ni Fe
1200 1000
1,5
800
Cu
600 A g 400
1,0
200 0
0
20 40 60 80 composition / [at% - Cu]
100
0,5
Cahn-Hilliard model 0
200
400
600
800
interface width / [nm]
Cu
temperature [°C]
1. 2.
0,0 1000
temperature / [K]
a)
b)
Figure 1: a) Atom probe analysis at Cu/Py multilayer after annealing at 400 °C interface: b) Thickness of intermixed zone versus annealing temperature. The inlay shows the phase diagram of CuAg.
107
Transmission Electron Microscopy Analysis of Tunnel Magneto Resistance Elements with Amorphous CoFeB Electrodes and MgO Barrier Michael Seibt1, Gerrit Eilers1, Marvin Walter1, Kai Ubben1, Karsten Thiel1, Volker Drewello2, Andy Thomas2, Günter Reiss2, and Markus Münzenberg1 1. Georg-August-Universität Göttingen, IV. Physikalisches Institut and Sonderforschungsbereich 602, D-37077 Göttingen, Germany 2. Fakultät für Physik, Universität Bielefeld [email protected] Keywords: MRAM, spin torque, amorphous/crystalline interface
Magnetic tunnel-junctions consisting of CoFeB/ MgO/ CoFeB trilayers have been of great interest in research just recently. Due to their high magnetoresistance they are a promising candidate for the fabrication of spintorque MRAM devices. For future writing concepts like current-induced magnetic switching, magnetic tunnel-junctions (MTJs) with thin barriers are necessary to provide sufficient high current densities. In such elements the tunnel magneto resistance (TMR) is strongly dependent on the electron transmission at the metal/oxide interfaces. Therefore the quality of the interfaces is of great significance and has to be optimized on the nanoscale. With the objective to correlate electrical transport properties (I-V characteristics, TMR) with the geometrical and chemical interface roughness, structural analysis was made by cross-sectional TEM and energy dispersive X-ray spectroscopy (EDX) in a Philips CM200-UT-FEG. Figure1 is a bright-field micrograph showing the multilayer stack grown on thermally oxidized silicon substrates. The heart of the device is the crystalline MgO barrier sandwiched between two CoFeB electrodes (see arrows in Figure 1). The atomic arrangement at the interfaces between electrodes and MgO barrier determine properties of spin transport across the barrier. The microstructure of this central part is characterized by a predominant interface roughness with a wavelength of about 10nm which may exceed the thickness of the barrier which is typically 2-2.5nm (Figure.2). Hence, for thicker TEM samples CoFeB electrodes and MgO barrier may overlap along the electron beam direction. Local crystallisation of the CoFeB electrodes is clearly revealed by high-resolution imaging. Due to the large roughness amplitude small-angle grain boundaries are observed in the MgO which predominantly grows in [100] direction. In addition, for non-working devices, cracking of MgO barriers is indicated by TEM. Although long-range ordering in CoFeB close to the MgO barrier is indicated in HREM images, the large interface roughness prevents a quantitative analysis on real devices. Films grown on crystalline MgO substrates with large atomically flat terraces indeed corroborate this hypothesis (see Figure 3). Post-growth thermal annealing indded shows that CoFeB cyrstallisation starts at interfaces to the MgO.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 107–108, DOI: 10.1007/978-3-540-85226-1_54, © Springer-Verlag Berlin Heidelberg 2008
108
Figure 1: Bright-field micrograph of a multilayer stack grown thermally oxidized silicon. Arrows indicate the functional part of the device, i.e. the crystalline MgO barrier between amorphous CoFeB electrodes.
Figure 2: Microstructure of the MgO barrier grown on a MnIr/CoFeB double layer as part of the multilayer stack shown in Fig.1. The predominant layer roughness has a wavelength of about 10nm and may exceed the barrier thickness of 2-2.5nm.
Figure 3: Amorphous CoFeB grown on (001) MgO substrate; the HREM image indicates long-range ordering in the CoFeB close to the substrate.
109
Study of the intermixing of Fe–Pt multilayers by analytical and high-resolution transmission electron microscopy W. Sigle1, T. Kaiser1, D. Goll1, N.H. Goo1, V. Srot1, P.A. van Aken1, E. Detemple2, and W. Jäger3 1. Max Planck Institute for Metals Research, Heisenbergstraße 3, D-70569 Stuttgart, Germany 2. Universität des Saarlandes, Postfach 151150, D-66041 Saarbrücken, Germany 3. Christian-Albrechts-Universität zu Kiel, Kaiserstraße 2, D-24143 Kiel, Germany sigle@mf mpg.de Keywords: EDXS, interdiffusion, multilayers
Materials used for advanced magnetic data storage devices must offer high magnetic anisotropy, high saturation magnetization, and an easy magnetization direction which is perpendicular to the array plane. These demands are fulfilled by the L10-ordered FePt. The most promising preparation technique for thin L10-ordered FePt films is deposition of Fe–Pt multilayers on MgO followed by thermal annealing. In this study we performed analytical [1] and in-situ high-resolution transmission electron microscopy (TEM) [2] studies on these multilayers. Five layers of Fe (6.4 nm thickness) and five layers of Pt (5.6 nm thickness) were alternately deposited on MgO substrates by ion beam sputtering. Cross-sectional TEM specimens were prepared by ion-beam milling. For the analytical studies, the TEM specimens were annealed in a TEM at different temperatures between 360 and 735 °C using a heating stage. Chemical concentration profiles were obtained by energydispersive X-ray (EDX) analysis in a VG HB501UX dedicated scanning TEM equipped with a Noran SYSTEM SIX EDX. In-situ high-resolution TEM (HRTEM) was done in the JEOL ARM1250. Ordered FePt phases are identified by the 0.37 nm spacing of the ordered {100} planes in HRTEM and by (100) reflections in diffraction patterns. The fully L10-ordered FePt structure, as obtained after annealing at 735 °C, is shown in Figure 1. At intermediate annealing temperatures also L12 phases (Fe3Pt and FePt3) are detected (not shown). These phases can be distinguished from the L10 phase by the appearance of ordering along two orthogonal directions. Figure 2 shows three EDX linescans obtained from the as-prepared material and from material annealed at 565 °C and 735 °C. The drop of the amplitude of concentration modulations is readily visible. After final annealing no modulations are detected any more. A plot showing the modulation amplitude as a function of annealing temperature is presented in Figure 3. It is found that the modulation amplitude decreases within 3 steps near 400, 600, and 700 °C. Using literature data of diffusion of Fe and Pt in various FePt systems, we found that the three annealing steps are related to the onset of diffusion (i) within pure Fe and Pt, (ii) within L12 phases, and (iii) within the L10 phase.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 109–110, DOI: 10.1007/978-3-540-85226-1_55, © Springer-Verlag Berlin Heidelberg 2008
110
1. 2. 3.
T. Kaiser, W. Sigle, D. Goll, V. Srot, P. A. van Aken, E. Detemple, and W. Jäger, J. Appl. Phys. (2008) in print. D. Goll, A. Breitling, N. H. Goo, W. Sigle, M. Hirscher, and G. Schütz, J. Iron Steel Res. Int. 13, Suppl. 1 (2006) 97. We kindly acknowledge the help of Ute Salzberger for TEM specimen preparation and R. Höschen and K. Hahn for technical assistance.
a
b Figure 1. High-resolution micrograph of the FePt multilayer after final annealing at 735 °C. The fringes belonging to ordered {100} planes are parallel to the MgO (100) substrate surface.
c
Figure 3. Normalized amplitude of the Pt concentration modulation after annealing. The data show averages and standard deviations of the three central Fe/Pt layers. Dotted lines mark plateau regions
Figure 2. Pt (---) and Fe (—) concentration across the Fe–Pt multilayer stack. (a) as prepared and after annealing at (b) 565 °C and (c) 735 °C.
111
Exploring structural dependence of magnetic properties in FePt nanoparticle by Cs-corrected HRTEM Z.L. Zhang1, J. Biskupek1, U. Kaiser1, U. Wiedwald2, L. Han2, P. Ziemann2 1. Materials Science Electron Microscopy, Ulm University, 89081 Ulm, Germany 2. Department of Solid State Physics, Ulm University, 89081 Ulm, Germany [email protected] Keywords: nanoparticles, Cs-corrector, HRTEM
Well-separated and size-controlled FePt nanoparticles are promising for magnetic data storages with ultra-high areal densities [1]. Chemically ordered L1o-FePt shows high magneto-crystalline anisotropy and an enhanced coercivity as compared to disordered FePt state. A measurement of coercivity (Hc) of FePt, showing strongly size dependence (shown in another paper), indicates a lower anisotropy when nanoparticle is small, which could be structural dependence. Newly-developed TEM techniques, Cscorrector and exit wave reconstruction, supplying less delocalized image, has enabled us to directly explore the structure of nanoparticle even with lateral dimension of only a few atoms[2]. In this work, an objective-lens Cs-corrected Titan FEI 80-300 microscope was used to explore the intrinsic structural characteristic of FePt particle with different sizes, and try to establish the structure-property relationship. In this study, all FePt particles were prepared by micellar approach [3-4], and followed by plasma etching treatment and reduction at 700°C. A series of representative HRTEM images with particle size ranges from 1.6 nm to 8.5 nm, recorded under a small Cs (less than 1 µm) and small over-focus, either cross-sectional (on MgO) or plan-view images, are shown in Figure 1. FFT from 2.3nm particle shows no superlattice reflections due to ordering. From the images, it is clearly seen that planar or line defects, i.e twin and dislocation, are dominant defects in these FePt particles, which lead to simply- and multiple-twinned particle. With the increase of particle size, the amounts of defect generally increase due to lattice mismatch, such as multiple twins in 7.2 nm and 8.5 nm particles, respectively. Epitaxial growth on MgO is possible only when the particle is smaller, i.e 1.6 nm, whereas it is lost as particle is larger, i.e. 6.0 nm, as a result, dislocations are usually introduced at interface or within the particle. The effective volume in the particle which contributes to magnetic moment could vary with the defect amount. Besides absence of ordering in smaller particles, the presence of these different types of defects in FePt particle may partially account for the observed magnetic properties. A statistic measurement and quantification about the relation of defect and particle size will be presented, further uncovering the intrinsic reasons for the demonstrated property. The stability of such FePt particle under electron beam and interface structure between FePt and MgO were investigated by both STEM and Cs-corrected HRTEM. Under STEM imaging, it is noted that Pt atom within a small FePt particle, i.e. 1~2 nm, is quite mobile. Closely examination on the behaviour of individual FePt under the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 111–112, DOI: 10.1007/978-3-540-85226-1_56, © Springer-Verlag Berlin Heidelberg 2008
112
beam reveals that atom cooperative movement in the particle occurs whereas the interface of FePt and MgO keeps quite stable due to a strong binding of Fe-O at the interface (Figure 2). Image simulations were conducted to prove the interfacial structure [5]. 1 2 3 4 5
O. Dmitrieva, et al, Phy.Rev B 76 (2007) 064414 R. M. Wang et al, Phy.Rev.Lett. 100, (2008)17205. U. Wiedwald et al , ChemPhysChem 6(2005)2522. G. Kästle et al, Adv.Funct.Mater., 13(2003)853. The authors thank the support from Germany Research Foundation DFG with SFB 569
Figure 1. HRTEM images of L1o-FePt nanoparticles recorded under Cs =1 µm , particle size is: (a) 1.6 nm, 2.3 nm with one twin and corresponding FFT is inserted, containing no superlattice reflections; (b) 4.0 nm, 2 twins; (c) 6.0nm, one edge dislocation in the particle; (d) 7.2 nm, five-fold twin, exit wave reconstructed phase image; (e) 8.5 nm, multiple twins. Note that the defect amounts are different in each particle.
Figure 2. A series of HRTEM images (FePt particle on MgO, viewed along [011], Wiener filtered) demonstrate under electron beam (0.042 A/mm2) the particle stability with exposure time, 0 s; 52 s and 280 s. It contains one twin boundary (indicated by arrow), atom cooperative movement along the boundary in the right part (three layer atoms) occurs.
113
Understanding the Chemistry of Molecules in Nanotubes by Transmission Electron Microscopy A.N. Khlobystov1,2, M.W. Fay2,3 and P.D. Brown2,3 1. School of Chemistry, University of Nottingham, Nottingham NG7 2RD, UK 2. Nottingham Nanoscience and Nanotechnology Centre, Nottingham NG7 2RD, UK 3. School of Mechanical, Materials and Manufacturing Engineering, University of Nottingham, Nottingham NG7 2RD, UK andrei [email protected] Keywords: nanotubes, fullerenes, TEM
Carbon Nanotubes (NTs) possess a spectrum of functional and exploitable properties such as high electrical and heat conductance, high tensile strength and superb thermal stability. One of the most fascinating physicochemical properties of nanotubes is their ability to host molecules due to their tubular topology [1-3]. The typical diameters of single-walled NTs range between 0.6 nm and 2 nm, and internal diameters of multiwalled NTs can reach 100 nm which makes carbon nanotubes ideal containers for a wide variety of molecular species. Several examples of templating action of nanotubes will be presented, and the underlying mechanisms of the nanotube-molecule interactions will be discussed. Most of the molecules interact with nanotubes via low-directional van der Waals forces. The most important parameter defining the efficiency of the NT-molecule interaction is the nanotube internal diameter. For spheroidal molecules, such as C60, the nanotube diameter controls the packing arrangement of the molecules (Figure 1). Most of the phases of C60 observed inside NTs do not exist in the free state and, therefore, are regarded as products of confinement in quasi-1D cavities of nanotubes. Various practical applications have recently been proposed for carbon nanotubes involved in non-covalent interactions with molecules, including sensors, photovoltaic devices and highly selective absorbents. One of the most fascinating developments in this area is the demonstration of chemical reactions inside nanotubes. The reactivity of molecules encapsulated in NTs can be controlled by this confinement. The nanotube in this case acts as a reaction vessel and a template for the reaction product, yielding unusual structures inaccessible by other means. One of the most illustrative examples is the controlled polymerisation of fullerene epoxide C60O recently carried out inside single-walled NTs [4,5]. Transmission electron microscopy (TEM) is the only direct method allowing visualisation of molecular structures inside carbon nanotubes. Positions and orientations of molecules can be visualised with atomic precision using TEM. The dynamic behaviour of molecules in nanotubes, such as translational and rotational motion, can also be monitored by taking time series TEM images. All this information is invaluable for the understanding of the effects of confinement in NT on the fundamental physicochemical properties of molecular species. The behaviour of the molecules may
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 113–114, DOI: 10.1007/978-3-540-85226-1_57, © Springer-Verlag Berlin Heidelberg 2008
114
be altered significantly as a result of irradiation with e-beam in TEM. The extent of these secondary effects depends crucially on the accelerating voltage and the imaging conditions which have to be tuned carefully to avoid artefacts associated with this technique. 1. D.A. Britz and A.N. Khlobystov, Chem. Soc. Rev. 35 (2006), p. 367. 2. A.N. Khlobystov, D.A. Britz and G.A.D. Briggs, Acc. Chem. Res. 38 (2005), p. 901. 3. http://www nottingham.ac.uk/nanocarbon/ 4. D.A. Britz, A.N. Khlobystov, K. Porfyrakis, A. Ardavan and G.A.D. Briggs, Chem. 5. 6.
Commun. (2005), p.37. A.N. Khlobystov in “Chemistry of Carbon nanotubes” American Scientific Publishers (2008), ISBN 1-58883-128-0 in press. We would like to acknowledge the EPSRC (UK), the European Science Foundation, the Royal Society and the University of Nottingham for financial support.
Figure 1. (a) Packing arrangement of fullerene C60 in the crystal. (b) High resolution transmission electron microscopy micrograph and a diagram of a C60@SWNT structure (nanotube diameter ~1.4nm). (c) Zigzag arrangement of fullerenes inside wide doublewalled carbon nanotube (inner diameter of the nanotube ~2.1nm).
115
Electrical and mechanical property studies on individual low-dimensional inorganic nanostructures in HRTEM D. Golberg1,2, P.M.F.J. Costa1, M. Mitome1, Y. Bando2 and X.D. Bai3 1. Nanoscale Materials Center, National Institute for Materials Science (NIMS), Namiki 1-1, Tsukuba, Ibaraki, 3050044, Japan 2. World Premier International Center for Materials Nanoarchitectonics (MANA), National Institute for Materials Science (NIMS), Namiki 1-1, Tsukuba, Ibaraki, 3050044, Japan, 3. Institute of Physics, Chinese Academy of Sciences, Beijing, 100080, China [email protected] Keywords: STM-TEM, AFM-TEM, nanotubes, nanowires, nanobelts
The present contribution demonstrates the recent advances achieved by the Group in pioneering studies of electromechanical properties of diverse low-dimensional individual inorganic nanomaterials inside a transmission electron microscope. The measurements were performed in high-resolution field-emission transmission electron microscopes operating at 300 kV, namely JEOL-3000F and JEM-3100FEF, and on freestanding individual nanoscale objects by means of specialized piezo-driven STM-TEM and AFM-TEM holders commercialized by “Nanofactory Instruments AB”. A sharp etched Au tip, acting as the STM tip, or a Si cantilever, as the AFM probe, was assembled within the holders (Figure 1 and Figure 2). Individual low-dimensional inorganic nanostructures were mounted on thin metallic (Au, Al) wires (Ø 250 μm), which may be piezo-driven in three dimensions (with a precision better than 1 nm). The successful experimental runs include multi-walled BN (Figures. 1,2) [1-4] and N-doped C nanotubes (NTs) [5,6], ZnO nanorods and nanowires [7], double-walled CNTs, multi-walled CNTs filled with Cu [8], Au, CuI or ZnS, inorganic nanothermometers, e.g. liquid Ga-filled MgO NTs and In-filled SiO2 NTs, CdS nanobelts, BN cones and so on. The current-voltage (STM-TEM, Figure 1) and/or force-displacement (AFM-TEM, Figure 2) curves were recorded under a full control of the nanomaterial morphological, crystallographic and chemical changes/transformations during all stages of probing/manipulation. This allowed us to unambiguously interpret many new intriguing physical, chemical and electromechanical phenomena peculiar to novel advanced nanostructures. These include, but are not limited to deformation-driven electrical transport and piezoelectricity in individual BNNTs, time-resolved electrical transport in N-doped CNTs, rheostat-like behaviour, femtogram (Cu) and attogram (CuI) mass transports, and nanopipetting in Cu- and Cu-halide-filled CNTs. 1. 2. 3.
D. Golberg et al., Adv. Mater. 19 (2007), p. 2413. D. Golberg et al., Nano Lett. 7 (2007), p. 2146. D. Golberg et al., Acta Mater. 55 (2007), p. 1293.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 115–116, DOI: 10.1007/978-3-540-85226-1_58, © Springer-Verlag Berlin Heidelberg 2008
116 X.D. Bai, D. Golberg et al., Nano Lett. 7 (2007), p. 632. P.M.F.J. Costa, D. Golberg et al., Appl. Phys. A 90 (2008), p. 225. P.M.F.J. Costa, D. Golberg et al., Appl. Phys. Lett. 91 (2007), p. 2231081. P.M.F.J. Costa, D. Golberg et al., J. Mater. Sci. 43 (2008), p. 1460. D. Golberg et al., Adv. Mater. 19 (2007), p. 1937. The authors are indebted to Dr. O. Lourie and Mr. K. Kurashima for a continuous technical support.
a1
a2
a4
a3
40 30
C urrent (nA )
4. 5. 6. 7. 8. 9.
20 10 0 -10
a1
-20
a2
-30
a3
-40
2 μm a
-50
b
a4
-20
-10
0
10
20
V oltage (V )
Figure 1. (a) Consecutive TEM images of an individual multi-walled BN nanotube bent inside HRTEM; and (b) the corresponding I-V curves recorded at different stages of the experiment (a1-a4). A notable current may pass through the nanotube in a bent state, while it disappears if the nanotube is unbent and straight.
Figure 2. Force-displacement curves directly recorded on a relatively thick (a) and a thin (b) individual multi-walled BN nanotube using an AFM-TEM setup. The insets display the nanotube appearance at different stages of the experiments.
117
Atomic structure of SW-CNTs: correlation with their growth mechanism and other electron diffraction studies R. Arenal 1, M.F. Fiawoo1, R. Fleurier1, M. Picher2, V. Jourdain2, A.M. Bonnot3, A. Loiseau1 1. LEM, CNRS-ONERA, 92322 Châtillon - France 2. LCVN, CNRS - Université Montpellier II, 34095 Montpellier - France 3. Institut Louis Néel CNRS/UJF, 38042 Grenoble - France Raul.Arenal@onera fr Keywords: Electron Diffraction, Atomic Structure, Growth Mechanism, Nanotubes, Nanofilaments
In this work, we have performed a comparative study of the helicity distribution in single wall carbon nanotubes (SW-CNTs) synthesized by different CVD processes in order to understand how the synthesis conditions can influence and control their growth mechanism [1]. To achieve this aim, we used the nano-beam (employing a parallel probe of about 50 nm) electron diffraction mode, which has been shown to be the most reliable technique for obtaining the complete determination of the atomic structure (chiral angle (θ) and diameter) of individual nanotubes (see for instance [2]). We recorded the intensities of electron diffraction patterns (EDPs) from individual SW-CNTs as well as from bundles of CNTs, using two different FEI Tecnai F20 TEMFEGs operating at 100 and 120 keV respectively. In the case of individual SW-NTs, their chiral indices were determined as the best value fitting experimental and simulated patterns calculated using kinematical electron theory. An example is shown in Figure 1 (a), which presents the EDPs of a SW-CNT, with in the inset the bright field image recorded under nanoprobe illumination of this tube. The structural parameters measured of this NT are θ=24.0 and diameter (extracted from the oscillations of the Eq-L) 2.8 nm. With these values, we simulate the corresponding EDPs and determined the chiral indices as the best fit between experimental and simulated EDPs. The SW-CNT of Figure 1 is thus unambiguously identified as a (24,17). In this contribution, we will present the comparative analysis of a significant number of NTs (>50) synthesized by two different CVD techniques: a thermal CVD process for which catalyst particles are prepared ex situ using a colloidal technique and deposited on the substrate and a hot filament CVD process where catalyst particles are prepared in situ by heating, under hydrogen gas, a few monolayers of the catalytic metal deposited on the substrate. In both cases, the substrates were perforated silica membranes, making possible to acquisition of EDPs from suspended nanotubes [1]. Furthermore, in this contribution we will also present our recent results on a very particular class of nano-filaments/NTs synthesized via CVD process. Figure 2 (a) shows a series of micrographs of a rope of 2 SW-CNTs and of their modification into a nanofilament. The analysis of the EDPs recorded on the rope section as well as on the filament section (Figure 2 (b) and (c), respectively) shows that we are dealing with two
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 117–118, DOI: 10.1007/978-3-540-85226-1_59, © Springer-Verlag Berlin Heidelberg 2008
118
different kinds of objects: NTs (on the left of the TEM images) and their transformation to another structure (on the right) which keeps constant the NTs’ chiral angle but loss their transitional periodicity and their cylinder shape. Our ongoing experiments and analysis on these very interesting objects will be also presented. 1. 2.
M.-F. Fiawoo A.-M. Bonnot, V. Jourdain, R. Arenal, J. Thibault, A. Loiseau, J. Nanoscience and Nanotec, to be submitted (2008). R. Arenal, M. Kociak, D.J. Miller, A. Loiseau, Appl. Phys. Lett, 89, 073104 (06).
Figure 1. (a) and (b) experimental and simulated EDPs of a SW-CNT (inset: bright field image), respectively. We assign these EDPs unambiguously to a (24,17) NT.
Figure 2. (a) TEM micrographs showing a rope of 2 NTs and their transformation to a nano-filament. (b) and (c) EDPs recorded on the rope and on the nano-filament, respectively.
119
TEM investigation ofSe nanostructures in/on Acetobacter xylinum cellulose gel-film N. Arkharova1, V.V. Klechkovskaya1, E. Suvorova1,2 1. A.V. Shubnikov Institute of Crystallography of Russian Academy of Sciences, Leninskii pr.,59, 119333, Moscow, Russia 2. Centre Interdisciplinaire de Microscopie Electronique, Ecole Polytechnique Federale de Lausanne, Station 12, CH-1015 Lausanne, Switzeland [email protected] Keywords: bacterial cellulose gel-film, polymer stabilised nanoparticles, selenium nanowires
Acetobacter xylinum cellulose (A X –BC) and its composites with some mineral and organic additives are the perspective materials for healing the heavy and complicated wounds. The Se/Ag/A X –BC composite is expected to have some antiphlogistic and immunostimulating properties [1]. This work reports the results of TEM/EDS analysis of the Se particles obtained from aqueous solutions by redox process in the presence of the N-poly (vinyl-2-pirrolidone) (PVP) and then absorbed by the surface and embedded into the AX BC gel-films. The PVP/Se ratio between 0 and 1 weight % was used. The solutions contained the traces of AgNO3. TEM images and SAED patterns, EDS data were processed and analyzed using Gatan Digital Micrograph 3.11.1, INCA (Oxford) and JEMS [2] software. TEM samples were the thin slices of the gel-film sections in epoxy. Two types of Se nanostructures were found: ellipsoidal particles in the range of sizes from 20 nm to 100 nm (Figure 1) and nanowires of a few nm width and up to a few microns long (Figure 2). Ellipsoidal particle were revealed both on the surface and ∼2 microns deep in the gel-film while the nanowires were only on the gel-film surface. X-ray EDS microanalysis and SAED patterns showed that ellipsoidal particles were the composites Se/ orthorhombic Ag2Se with different ratio between Se and Ag2Se. Nanowires had the structure of trigonal Se and appeared only in the solution with the Se concentration higher than 0.5% PVP/Se. 1. 2. 3.
Yu. G. Baklagina, A.K. Khripunov et al. Russ. J. Appl. Chem. V. 78 (2005) P. 1176-1181 P. Stadelmann, JEMS. http://cimewww.epfl.ch/. 2008. We kindly appreciate to our colleagues from Institute of Macromolecular Compounds, RAS, for given samples.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 119–120, DOI: 10.1007/978-3-540-85226-1_60, © Springer-Verlag Berlin Heidelberg 2008
120
Figure 1. TEM image of the Se/Ag/A X-BC composite cross-section in epoxy
Figure 2. TEM image of selenium nanowires
121
In-situ electron irradiation studies of metal-carbon nanostructures L. Sun1, Y. Gan1, J.A. Rodriguez-Manzo2, M. Terrones3, A.V. Krasheninnikov4 and F. Banhart2 1. Institut für Physikalische Chemie, Universität Mainz, D-55099 Mainz, Germany 2. Institut de Physique et Chimie des Matériaux, UMR 7504, F-67034 Strasbourg 3. Advanced Materials Department, IPICyT, 78216 San Luis Potosí, México 4. Accelerator Laboratory, University of Helsinki, P.O.B. 43, FIN-00014, Finland [email protected] fr Keywords: nanotubes, carbon, in-situ electron microscopy
The properties and the behaviour of nanoparticles are subjects of highest current importance. Experiments on individual clusters are generally difficult but can be carried out by the techniques of modern in-situ electron microscopy. The electron beam can be used as a tool to induce structural changes on an almost atomic scale [1]. Particularly well-suited systems for electron irradiation studies are metal nanocrystals in graphitic shells. Under electron irradiation, the shells contract and lead to compressive forces. By measuring the lattice spacings in HRTEM images of metal crystals inside graphitic shells, pressures on the order 10-20 GPa were determined [2]. Nonhydrostatic pressure, e.g., inside collapsing nanotubes, may deform the crystals considerably. This can be made use of for studying the deformation behaviour of individual nanometer-sized crystals. Figure 1 shows how a Co wire inside a carbon nanotube is deformed and extruded when the nanotube collapses locally under electron irradiation [3]. Another deformation cell, allowing the detailed study of crystal deformation, was designed by electron-beam structuring, as shown in figure 2. A 'carbon onion', encapsulating a Au crystal, was punctured by a fully focused electron beam and subsequently exposed to uniform irradiation so that the Au crystal was slowly extruded through the hole. The experiment was carried out at different temperatures and with different metals, and the deformation of metal crystals was studied in detail [4]. Electron irradiation of metal-carbon nanocomposites leads to the ballistic displacement of atoms from the graphitic shells. Some carbon atoms are sputtered into the metal crystal and may, depending on the solubility and diffusivity of carbon in the respective metal, segregate at the metal surface. This is shown in figure 3 where carbon atoms are ingested into a FeCo crystal in a multi-wall carbon nanotube [5]. A new nanotube nucleates and grows through the channel of the host nanotube. This experiment allows us to study the nucleation and growth of nanotubes by in-situ electron microscopy. The interaction between metal and carbon was also studied on an atomic scale by introducing Au and Pt atoms into graphene layers. Individual Au or Pt atoms were observed by HRTEM at different temperatures, and their migration was monitored [6]. [7] 1.
A. Krasheninnikov and F. Banhart, Nature Materials 6 (2007) 723.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 121–122, DOI: 10.1007/978-3-540-85226-1_61, © Springer-Verlag Berlin Heidelberg 2008
122
2. 3. 4. 5. 6. 7.
L. Sun, J.A. Rodriguez-Manzo and F. Banhart, Appl. Phys. Lett. 89 (2006) 263104. L. Sun, F. Banhart, A. Krasheninnikov, J.A. Rodriguez-Manzo, M. Terrones and P.M. Ajayan, Science 312, (2006) 1199. L. Sun, A. Krasheninnikov, T. Ahlgren, K. Nordlund and F. Banhart, submitted. J.A. Rodriguez-Manzo, M. Terrones, H. Terrones, H.W. Kroto, L. Sun and F. Banhart, Nature Nanotech. 2 (2007) 307. Y. Gan, L. Sun and F. Banhart, Small, in the press. Support by the DFG (Ba 1884/4-1) is gratefully acknowledged.
Figure 1. Electron irradiation of a carbon nanotube encapsulating a Co crystal. The collapse of the tube leads to the extrusion of the metal [3].
Figure 2. Extrusion of a Au crystal through a focused-beam-induced hole (top left) from a spherical carbon shell under subsequent uniform electron irradiation [4].
Figure 3. Growth of a multi-wall carbon nanotube (arrowed) from a FeCo crystal inside a host nanotube under uniform electron irradiation [5].
123
Application of 80kV Cs-corrected TEM for nanocarbon materials A. Chuvilin1, U. Kaiser1, D. Obergfell2, A. Khlobystov3, S. Roth2 1. University of Ulm, Central Facility of Electron Microscopy, Electron Microscopy Group of Materials Science, Albert Einstein Allee 11, 89069 Ulm, Germany. 2. Max Planck Institute for Solid State Research, Heisenbergstraße 1, 70569 Stuttgart, Germany. 3. School of Chemistry, University of Nottingham, University Park, Nottingham NG7 2RD, UK. [email protected] Keywords: TEM, Cs correction, carbon materials
Being one of the main methods for studying the atomic structure of carbon materials, high resolution TEM suffers from a serious flaw as the energy of electrons, necessary to obtain atomic resolution (200-300 keV), is far above the kick-off damage threshold for graphitic carbon (about 60 keV) [1], which means that carbon nanostructures are always observed with a structure more or less distorted by electron beam. Practical implementation of Cs correctors in the last decade [2] opened the possibility to decrease acceleration voltage of the microscopes significantly, yet preserving the resolution at reasonable level. Decreasing the energy of the electron beam, besides decreasing radiation damage, has the advantage of increasing the phase contrast [3]. Considering the possibility to visualize one single carbon atom, the increase of the contrast reduces quadratically the electron dose necessary for this. Here we report our first experience in application of 80kV electron microscope with imaging Cs corrector (Titan 80-300, FEI, Holland) for studying carbon nanotubes, peapods and graphene. We show that nano-structures composed of graphitic carbon are stable under the conditions of observation for more than 30 minutes, that opens the possibility for monitoring of single atom dynamics, diffraction studies and EELS measurements without radiation damage induced by the electron beam. Visualization of one single carbon atom within a graphene network is electron-optically achievable, but is limited in a single shot by the dynamical range of the CCD camera. Thus a multiple frame acquisition-averaging method is proved to be adequate for accumulation the electron dose necessary for resolving single carbon atom. Direct visualization of defects within the graphene network is demonstrated (Figure 1); in particular the stability of a mono-vacancy is shown under the beam irradiation. Though almost eliminating kick-off damage unavoidable at medium range electron energies, decreasing the energy to 80keV significantly increase ionization and heating of the sample. Ionization is not an issue for graphitic carbon materials due to high electrical conductivity, while special precautions should be taken against local overheat. From the other hand side the elevated temperature inside the beam spot opens possibilities for dynamical observation of heat activated chemical reactions and
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 123–124, DOI: 10.1007/978-3-540-85226-1_62, © Springer-Verlag Berlin Heidelberg 2008
124
structure transformations. On the example of a heat induced transformation of SWNT peapod into double wall nanotube it is shown that good heat sink is essential for observation of pristine atomic structure of sensible materials at low voltages. At the conditions, when an area under observation is thermally isolated, heat induced evolution of the structure of SWNT metallofullerene peapods is observed, namely: breakage of the walls and coalescence of fullerene balls, behavior and interaction of individual metal atoms, inner tube formation from fullerenes, coalescence and collective action of Dy atoms resulting in SWNT breakage, self curing of the tube. At similar conditions the dynamics of Ag atoms on the surface of graphene is monitored. A formation of unusual 2D surface crystals with 4-fold symmetry is shown. Utilization of accelerating voltages below 100kV at Cs corrected TEM opens possibilities for a broad field of research of pristine atomic structure of materials including light elements like carbon and point defects like single vacancies. 1. 2. 3.
R.F. Egerton, P. Li, M. Malac, Micron 35 (2004), p. 399. M. Haider, H. Rose, S. Uhlemann, E. Schwan, B. Kabius, K. Urban, Ultramicroscopy 75 (1998), p. 53. M.T. Hayashida, T. Kawasaki, Y. Kimura, Y. Takai, Nuclear Inst. and Methods in Physics Research 248 (2006), p. 273
Figure 1 Monovacancy in a single graphene sheet. (a) Overview of graphene edge. The image is a drift corrected average of 10 frames. (b) Simulated image and (c) a model of monovacancy. Image is calculated for the conditions of the best visibility of the vacancy (Cs=-10μm, df=-8nm). (d) Simulated image considering electron dose of 106e-/nm2 (top) and experimental image obtained by single 1 sec exposition (bottom). (e) The same set as (d), but for the dose 107e-/nm2 and 10 frames average correspondingly.
125
Control of gold surface diffusion on Si nanowires Martien .I. den Hertog1, Jean-Luc. Rouviere1, Florian Dhalluin2, 3, Pierre J. Desré3, Pascal Gentile4, Pierre Ferret3, Fabrice Oehler4, Thiery Baron2 1. Laboratoire d'Étude des Matériaux par Microscopie Avancée, CEA/DRFMC, CEAGrenoble, 17 rue des Martyrs, 38052 Grenoble Cedex 9 2. Laboratoire des Technologies de la Microélectronique, CNRS UMR 5129, CEAGrenoble 17 rue des Martyrs, 38052 Grenoble Cedex 9 3. Laboratoire de Photonique sur Silicium, CEA/LETI/DOPT, CEA-Grenoble 17 rue des Martyrs, 38052 Grenoble Cedex 9 4. Laboratoire Silicium Nanoélectronique Photonique et Structure, CEA/DRFMC, CEA-Grenoble, DRFMC, 17 rue des Martyrs, 38052 Grenoble Cedex 9 [email protected] Keywords: Silicon nanowires, STEM, Gold diffusion
Silicon nanowires (NW) were grown by the Vapour-Liquid-Solid (VLS) mechanism using gold as the catalyst and silane as the precursor. In this work we show that the diffusion of gold from the catalyst particle over the wire sidewalls can be controlled by adjusting growth parameters: partial silane pressure and growth temperature. The diameter of the NWs has also an effect. Gold diffusion results in the formation of gold clusters on the wire sidewalls (Figure 1). High Angle Annular Darkfield Scanning Transmission Electron Microscopy (HAADF STEM) and Scanning Electron Microscopy (SEM) were used to observe the presence or absence of gold clusters on the wire sidewall. In literature an influence of oxygen on the gold diffusion can be found [1]. Figure 2 illustrates the effect of growth temperature and partial silane pressure on the gold surface diffusion. Gold clusters are absent on the NW side walls for high silane partial pressure, low temperature and small NW diameters. The NW sidewall morphology is modified by the presence of gold. Different models will be qualitatively discussed in the presentation. The adsorption of silane on the NW sidewalls seems to be the main physical effect governing gold diffusion. 1. 2.
S. Kodambaka, J. B. Hannon, R. M. Tromp, F. M. Ross, Nano Lett. 6 (2006), 1292 The results reported in this publication were obtained with research funding from the European Community under the FP6 - Marie Curie Host Fellowships for Early Stage Research Training (EST) “CHEMTRONICS” Contract Number MEST-CT-2005-020513
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 125–126, DOI: 10.1007/978-3-540-85226-1_63, © Springer-Verlag Berlin Heidelberg 2008
126
Figure 1. High resolution HAADF STEM image showing the gold clusters on the NW sidewall, the brighter particles are gold.
Figure 2. (A) SEM image of a wire grown at 500°C at low partial silane pressure (0.19 mbar) clearly covered by gold clusters and slightly tapered. (B) HAADF STEM image of a wire grown at 430°C at low partial silane pressure (0.19 mbar); gold clusters can be observed near the catalyst particle. (C) HAADF STEM image of a wire grown at 500°C at high partial silane pressure (1.023 mbar). Gold clusters can be observed on the 300 nm region close to the catalyst particle.
127
Nanowires of Semiconducting Metal-oxides and their Functional Properties M. Ferroni1, C. Baratto1, E. Comini1, G. Faglia1, L. Ortolani2,3, V. Morandi2, S. Todros1, A. Vomiero1, and G. Sberveglieri1 1. INFM-CNR SENSOR and Dept. of Chemistry and Physics, Brescia University, via Valotti 9, 25133 Brescia, Italy 2. CNR-IMM Section of Bologna, via Gobetti 101, 40129 Bologna, Italy 3. University of Bologna, Dept. of Physics, v.le B. Pichat, 6/2, 40127 Bologna, Italy. [email protected] Keywords: Indium oxide, tin oxide, biosensor.
The increasing scientific interest in crystalline nanowires and nanorods has stimulated their functional exploitation, and single-crystalline nanowires are nowadays emerging as building blocks for a new generation of electronic [1,2,3], and optoelectronic nanometer-scaled devices [4,5]. The structural and functional properties of nanostructures of ionic metal oxides are attracting almost the same consideration addressed to nanowires of silicon or group III-V compounds. The synthesis of tin- and indium- oxides nanowires is based on thermal decomposition of precursor powders followed by vapor-solid (VS) or vapor-liquid-solid (VLS) growth. Such a process is very promising for nanostructure fabrication, due to its simplicity with respect to the top-down technology of silicon processing. Microstructural investigation of the nanowires is a key-feature for a thorough knowledge of the growth mechanisms, which can be assisted by either seeding particles or noble metal catalysts (see Figure 1), enhancing the capability to control the dimension and the shape of the nanostructures [6]. The chemical homogeneity and the crystalline arrangement were investigated by SEM and TEM. HRTEM and electron diffraction revealed the single-crystal arrangement and the atomically-sharp crystal facets for the termination of the nanowires. EDX and STEM were used for the investigation of impurities and local variations in the composition. Further improvement of the preparation methodology addresses the capability to fabricate heterogeneous structures and chemically non-homogeneous nanowires. As shown in Figure 2, the transport and condensation process was tailored to obtain a longitudinally-assembled heterostructure of In2O3 and SnO2 [7]. The nucleation and growth of single-crystalline SnO2 nanowire at the termination of an In2O3 nanowire was obtained through the prominent catalytic activity of gold nanoparticles. For the investigation of the electrical properties of nanowires, piezo-actuated manipulators were operated into the SEM to fabricate single-wire-based devices. Presently, nanowires of tin oxide are presently under exploitation for applications in the field of chemical sensing and DNA detection.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 127–128, DOI: 10.1007/978-3-540-85226-1_64, © Springer-Verlag Berlin Heidelberg 2008
128
1. 2. 3. 4. 5. 6. 7.
Y. Cui and C.M. Lieber, Science 291 (2006) p. 851. X.Duan et al, Nature 409 (2001) p. 66. Y. Huang et al, Nano Letters 2 (2002) p. 101. C.M. Lieber, MRS Bullettin 28 (2003) p. 486. L. Samuelson et al, Materials Today 6 (2003) p. 22. A. Vomiero Crystal Growth and Design 7 (2007) p. 2500. A. Vomiero et al., Nano Letters 7 (2007) p. 3553.
Figure 1. (left) Nucleation and growth of In2O3 nanowires from the In2O3 buffer layer over a sapphire substrate. (right) TEM image of the catalytic gold particle at the tapered apex of a crystalline In2O3 nanowire prepared by VLS.
Figure 2. Structural characterization of the longitudinal In2O3-SnO2 heterostructure. (main picture) TEM panoramic view of the In2O3 nanowire, with the SnO2 nanowire extending lengthwise. The black arrow marks the termination of the SnO2 nanowire and the catalytic Au nanoparticle, which assisted the VLS growth of heterostructure. (1) SAED pattern showing the cubic single-crystal arrangement for the indium oxide nanowire. (2) CBED pattern and High-Resolution image from the tin oxide nanowire, demonstrating its single-crystalline cassiterite arrangement. (3-4) highly magnified TEM view and corresponding SAED pattern of the heterojunction, where superimposition of both indium and tin oxides has been recorded.
129
Phase relations in the Fe–Bi–O system under hydrothermal conditions A. Gajović1, 2, S. Šturm1, B. Jančar1, M. Čeh1 1. Jožef Stefan Institute, Jamova 39, SI-1000 Ljubljana, Slovenia, 2. Ruđer Bošković Institute, Bijenička 54, HR-1002 Zagreb, Croatia, [email protected] or gajovic@irb hr Keywords: hydrothermal synthesis, bismuth ferrite, hematite, goethite, bismuth oxide
The phases appearing during a hydrothermal reaction in the Fe–Bi–O system were investigated, with the aim to optimize the conditions for the syntheses of nanostructured bismuth ferrite. BiFeO3 is a multiferroic material; hence it is ferroelectric and antiferromagnetic at room temperature [1]. Since the spins in this material take the form of a long-wavelength (62 nm) the spiral linear magnetoelectric effect averages to zero. One of the ways to recover this linear effect is with thin-film epitaxial constraints. Thus, we expect the same effects in nanostructured BiFeO3. For the hydrothermal reactions two different precipitation procedures were carried out with various molar ratios (x) of iron and bismuth ions. In the first procedure the solutions containing both iron and bismuth ions (starting compounds Fe(NO3)3·9H2O and Bi(NO3)3), were co-precipitated with tetraethyl ammonium hydroxide (TMAH), while in the second procedure the precipitation of the iron and bismuth ions was carried out separately, prior to mixing in the autoclave. Before the precipitation the Bi(NO3)3 was dissolved in HNO3 by vigorous stirring. The hydrothermal treatments were performed in the autoclave at pH 13.54 at 200°C for 6 h. The stability of the phases was checked in the case of 10 mol% Bi(NO3)3 by one week of hydrothermal treatment. The prepared phases were analyzed by X-ray powder diffraction (XRD), while the morphologies and nanostructure of the different phases were determined using highresolution transmission electron microscopy (HRTEM) and/or scanning electron microscopy (SEM). The chemical compositions were examined by energy-dispersive Xray analysis (EDXS). The phases observed in the prepared samples are listed in Table I. The tailoring of the goethite morphology in both series of precipitations was investigated by TEM. It was observed that the aspect ratio of goethite nanorods increased with the increase of Bi3+ ions in the reaction. However, other phases, like hematite and bismuth ferrite, were also produced. We obtained pure bismuth ferrite only in a co-precipitated sample with x=50%. In the case of separate precipitation, BiFeO3 was produced in a reaction with a lower content of Bi3+. Again, various phases coexisted in the sample. Goethite and hematite were shown to be stable phases (Figure 2). In hematite, containing approximately 7.2% of Bi3+, stacking faults were observed (Figure 2b). These are potential sites for Bi3+ accommodation, thus indicating a possible mechanism for the synthesis of nanosized BiFeO3.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 129–130, DOI: 10.1007/978-3-540-85226-1_65, © Springer-Verlag Berlin Heidelberg 2008
130 1. 2.
W. Eerenstein, N. D. Mathur and J. F. Scott, Nature 442 (2006), p. 759. The authors acknowledge financial support from the European Union under the Framework 6 program under a contract for an Integrated Infrastructure Initiative. Reference 026019 ESTEEM.
Table I. The phases obtained with hydrothermal reactions based on the XRD analysis. x indicates mol% of Bi3+ in the reaction. x (mol %) Bi+3 2
5
10
20
30
50
Co-precip.
G*
G
G, H*
G
G, Bi25FeO40
G, BiFeO3, Bi2O3
G, H, BiFeO3 G, H BiFeO3, Bi2O3
BiFeO3
Separate precip.
amorph. phase G, H, BiFeO3, Bi2O3
H, BiFeO3, Bi2O3
10 (one week)
G, H
* G→goethite (α-FeO(OH)); H→hematite (α-Fe2O3)
a)
b)
Figure 1. a) Bismuth ferrite hydrothermally synthesized in a co-precipitated sample with x = 50 %. b) High-resolution micrograph of synthesized BiFeO3. a)
b) H
G
Figure 2. a) Goethite nanorods (G) and hematite (H) as stable phases after one week of the hydrothermal reaction. b) HRTEM of hematite with stacking faults (denoted by arrow).
131
Dose dependent crystallographic structure of InAs nanowires F. Gramm1, E. Müller1, I. Shorubalko2, R. Leturcq2, A. Pfund2, R. Wepf 1 and K. Ensslin2 1. Electron Microscopy ETH Zurich – EMEZ, 2. Laboratory of Solid State Physics Swiss Federal Institute of Technology - ETHZ, CH-8093 Zurich, Switzerland [email protected] Keywords: InAs nanowires, transmission electron microscopy, crystal structure
Semiconductor technology has improved the procedures to miniaturize devices step by step. Usually these devices are produced by lithographic methods on planar substrates. Another approach is to grow nano-objects, which could then be assembled to an electronic device ‘bottom-up’ as discussed in [1,2]. The InAs-nanowires investigated in this study were grown by Metal-Organic Vapor Phase Epitaxy (MOVPE) on a GaAs 〈111〉B substrate. The wires were grown catalytically from gold nanoparticles, which were randomly distributed on the substrate, as it was first performed and described by Wagner and Ellis [3]. The crystallographic structure of semiconductor nanowires is one of the important properties, which determine the electronic or optical properties of these miniaturized devices. To explore the structural organisation, nanowires were investigated by HRTEM (FEI Tecnai F30 FEG; 300kV, point to point resolution 0.19nm). The InAs nanowires crystallise in zinc-blende or in wurzite structure, which are the two maximally closedpackings for InAs. Selected area electron diffraction (SAED) was used to determine which of the two structures was present in the analysed nanowires. The nanowires, grown as described by A. Pfund et al. [4], were found to have mainly wurzite structure as confirmed by high-resolution electron microscopy (HRTEM) (Figure 1). In additions a small approximately 3nm thick amorphous oxide layer covering the surface of the nanowires was found.. No defects in the crystal lattice were visible in the first exposure during HRTEM imaging. However on the following exposure (Figure 2), taken some minutes later from the same area of the nanowire, lattice fringes were also observed in the oxide layer. Further increase of the electron dose resulted in a more and more complete distortion of the nanowire. A patchwork of lattice fringes became visible in HRTEM images and at some positions of the nanowire even zinc-blende SAED-pattern as shown in Figure 2 were obtained, which could not be found under low dose exposure. It is well known that electrons interact strongly with matter and can therefore also change or damage samples. Here we show that the electron irradiation may change the structure of nanowires. From the SAED pattern it is also clear, that both wurzite and zinc-blende structure occur in these nanowires. Due to the fact that the SAED-pattern of the zinc-blende structure was only observed after extended irradiation, it may be that the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 131–132, DOI: 10.1007/978-3-540-85226-1_66, © Springer-Verlag Berlin Heidelberg 2008
132
zinc-blende type structure represents only transformed wurzite type structures from non irradiated nanowires. To be on safe side for structure investigations of e.g. sensitive nano-devices it will be necessary to record a pair of images - one at minimal dose and one at extended irradiation - to document beam induced material reorganisation. 1. 2. 3. 4.
C.M. Lieber, Sci. Am. 285 (2001), p.58. W. Lu, C.M. Lieber, Nature Materials 6 (2007), p. 841. R.S. Wagner, W.C. Ellis, Appl. Phys. Lett. 4 (1964), p. 89. A. Pfund et al., Chimia 60 (2006), p. 729.
Figure 1 HRTEM-image of InAs-nanowire. A) Nanowire cover with the small oxide layer. Some lattice fringes can be recognized in the oxide layer and a Moirée-pattern of two overlapping crystal lattices is visible in the nanowire. B) SAED-pattern of wurzite structure with viewing direction along 110. C) HRTEM-image of the InAs showing a patchwork of lattice fringes. D) The zinc-blende SAED-pattern which can be observed after some working time e.g. in such a distorted nanowire.
133
HRTEM simulations of planar defects in ZnTe nanowires I. Häusler1, H. Kirmse1, W. Neumann1, S. Kret2, P. Dłużewski2, E. Janik2, G. Kraczewski2, and T. Wojtowicz2 1. Humboldt University of Berlin, Insitute of Physics, D-12489 Berlin, Germany 2. Institute of Physics PAS, Al. Lotników 32/46, 02-668 Warsaw, Poland haeusler@physik hu-berlin.de Keywords: nanowire, HRTEM simulation, vapour-liquid-solid growth
Semiconductor nanowires are freestanding one-dimensional objects with a length of some microns and a diameter of few tens of nanometres. Due to this unique shape the electronic states of the nanowires are quantized perpendicularly to the growth direction. Such semiconductor structures are favourable for numerous applications. However, semiconductor nanowires very often contain planar defects. In order to prevent defects during the growth process it is very important to have a thorough understanding of their nature and formation. In this work we have investigated the structure of ZnTe nanowires grown on (001) oriented GaAs substrate by vapour-liquidsolid (VLS) deposition. A liquid droplet of gold with a sphere size of about 70 nm acts as a catalyst and defines the diameter of the beneath growing nanostructure during the molecular beam epitaxy. The defects were analysed by high-resolution transmission electron microscopy (HRTEM). Figure 1 shows a bright-field TEM image of a separated ZnTe nanowire on a holey carbon film. For the defect analysis HRTEM images were interpreted by computer simulation. Figure 2 is a HRTEM image observed in a [01-1] zone axis orientation of the nanowire. The planar defects are visible by the characteristic lines perpendicular to the <111> growth direction. On the basis of the HRTEM images the planar defects can be identified as stacking faults with {111} stacking fault planes. In the field of view, the orientation of the dumbbells is flipping from one lamella to the next lamella. The mean thickness of the lamellae varies from two to six monolayers (MLs). It seems that one orientation is more favourable than the other. We assume that these lamellae were formed by rotational twinning, where a 180° rotation around the [111] nanowire axis takes place. For HRTEM image simulation we constructed a super cell containing a twin lamella with a thickness of three MLs (cf. Figure 3). Figure 4 shows the results of the HRTEM image simulation as a function of the specimen thickness and the defocus values. The comparison of the experimental HRTEM image (Figure 2) and the simulated image of the super cell containing the twin lamella (Figure 3) reveals a good agreement for specimen thicknesses between 90 Å and 110 Å and defocus values between -120 Å and -170 Å. Both images show the zigzag pattern of the flipping dumbbells. In addition, HRTEM simulation will be presented where the influence of the cylindrical shape of the nanowire as well as astigmatism and defocus variation were considered.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 133–134, DOI: 10.1007/978-3-540-85226-1_67, © Springer-Verlag Berlin Heidelberg 2008
134
Figure 1: Bright-field image of an isolated ZnTe nanowire on a holey carbon film.
Figure 2: HRTEM image of upper region of a ZnTe nanowire (cf. marked area in Fig. 1).
Figure 3: Super cell for HRTEM simulations
Figure4: Results of the HRTEM image simulation for the super cell shown in Fig. 3
135
A universal method for determination of helicities present in unidirectional groupings of graphitic or graphitic-like tubular structures H. Jiang1, D.P. Brown2, A.G. Nasibulin1 and E.I. Kauppinen1,3 1. Laboratory of Physics and Center for New Materials, Helsinki University of Technology, P.O. Box 5100, 02150 Espoo, Finland 2. Canatu Ltd., Tekniikantie 21, 02150 Espoo, Finland 3. VTT Biotechnology, Technical Research Center of Finland, 02044 VTT, Finland [email protected] Keywords: electron diffraction, helicity, nanotubes
Since the recognition of carbon nanotubes by Iijima in 1991, nano-scale tubular structures, including graphitic carbon nanotubes (CNTs) and graphitic-like boron-nitride nanotubes (BNNTs), have generated tremendous research and engineering interest because of their unique helical structures as well as extraordinary properties. The physical properties of nanotubes sensitively depend on their helicities. Applicationoriented research on tubular structures thus requires reliable control over the growth process for selectively forming nanotubes with desired helicity. To better understand properties, develop practical applications and control synthesis, it is crucial to advance our capability for structural characterization of nanotubes. It has been widely recognized that electron diffraction is a powerful technique for structural characterization of nanotubes with little constrains in contrast to other tools like optical measurements. Electron diffraction analysis of individual single-walled CNTs [1, 2] or BNNTs [3] enables explicit determination of their atomic structures specified by so-called chiral indices (n,m). In reality, nanotubes often form bundles, or exist as coaxial multi-walled tubes, i.e. in general, in the form of unidirectional groupings, rather than as individual tubes. However, current solutions for structural characterization of such groupings are far from adequate and there is an urgent need for a reliable and quantitative method to characterize structural helicity properties in realistic samples. Here we introduce a universal method [4] for complete determination of helicities present in multi-walled or bundled carbon or boron-nitride nanotubes or their structural analogs. A critical dimension characteristic of the structural property of the atomic bond length in the structures is discerned from their electron diffraction patterns (EDPs), by which, all helicities present in the groupings of nanotubes are identified. The method is illustrated by using a simulated EDP of a single-walled CNT bundle (Figure 1) containing four tubes (13,2), (18,7), (20,6), (26,6). The diffraction pattern was calculated using the DIFFRACT program [5] by assuming a bundle tilt angle of 15° with respect to the electron beam. Eventually all helicities present in the bundle have been successfully resolved with an accuracy better than 0.2°.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 135–136, DOI: 10.1007/978-3-540-85226-1_68, © Springer-Verlag Berlin Heidelberg 2008
136
The method is further applied successfully for helicity analysis of two multi-walled BNNTs from their experimental electron diffraction patterns shown in Figure 2, which are reproduced with permission from A. Celik-Aktas et al, Applied Physics Letters, 86, 133110 (2005).Copyright 2005, American Institute of Physics. The results show precise details about the existing or missing helicities in the structures. A further application of the introduced method has been made to CNTs synthesized in a laser oven and has disclosed interesting structural phenomena. This will also be presented. 1. 2. 3. 4. 5. 6.
H. Jiang, A. G. Nasibulin, D. P. Brown and E. I. Kauppinen, Carbon, 45 (2007), p. 662. M. Gao, J.M. Zuo, R.D. Twesten, I. Petrov, L.A. Nagahara and R. Zhang, Appl. Phys. Lett. 82 (2003), p.2703 . R. Arenal, M. Kociak, A. Loiseau and D.-J. Miller, Appl. Phys. Lett. 89 (2006), p. 073104 H. Jiang, D. Brown, A.Nasibulin and E.I. Kauppinen, Phys. Rev. Lett. (2008), submitted. Ph. Lambin and A. Lucas, Phys. Rev. B 56 (1997), p.3571. We kindly acknowledge financial support from the Academy of Finland.
Figure 1. A simulated electron diffraction pattern of a SWCNT bundle containing four individual tubes (13, 2), (18, 7), (20, 6) and (26. 6).
Figure 2. Electron diffraction patterns from multiwalled BNNTs with (a) a narrow range of chiral angle distribution; and (b) a wide helicity distribution. The presence of the layer-line gap "A", "B" and "C" in (b) indicates deficiencies of certain helicities in the multiwalled nanotube, which has been evaluated.
137
Microstructure of (112) GaAs nanorods grown by MBE E. Johnson1,2, S.A. Jensen1, L.P. Hansen1, C.B. Sørensen1 and J. Nygård1 1. Niels Bohr Institute, Nano Science Center, University of Copenhagen, Denmark 2. Department of Materials Research, Risø DTU, Roskilde, Denmark [email protected] Keywords: GaAs, Nanowires, TEM
Semiconductor nanorods of GaAs have been grown by MBE technique on (100) GaAs wafers. Au nanoparticles acting as nucleation and catalyst sites were made on the oxide free wafers by evaporation at 660 °C. After annealing for 10 minutes in an As backing flux, growth of the nanorods was carried out at 515 °C, and during final cooling of the samples to room temperature the As flux was maintained. Most of the nanorods were found to grow along the As-terminated (111)B directions typically with a heavily faulted zincblende structure or with larger perfect segments of wurtsite separating faulted zincblende segments [1]. This is the same growth and microstructure morphology observed for GaAs rods grown on (100) substrates using gold-particle-assisted metal-organic vapour-phase epitaxy [2]. However, in the present experiments a small fraction – about 5% – of the nanorods were found to grow in directions different from (111)B. Using a cleaved wafer it was possible from the knowledge of the wafer geometry to make a geometric analysis in the SEM of these rods which were found to grow along the (112)A directions (Figure 1). The (112) rods often appear to have special lancet-shaped blade-like microstructure where one part of the blade has a very smooth and straight edge. This part has wurtzite structure with the (11-20) direction parallel to the blade and rod axis. The other part has a more irregular and rugged edge and the crystallographic structure is zincblende with the (112) direction parallel to the blade and rod axis (Figure 2). In other cases the (112) rods would have a perfect wurtzite structure containing lamellae of zincblende a few monolayers in thickness parallel to the rod axis (Figure 2 and 3a). The zincblende parts of the rods in general contain more defects in form of intersecting stacking faults, twin lamellae and occasional appearance of wurtzite segments (Figure 2 and 3b). Minority formation of unusual nanorods may be due to local differences in the growth conditions either from defects in the wafer surface or as suggested by Wu et al. [3] as due to local strain variations. This should be studied further to elucidate details in the growth processes leading to occurrence of anisotropic crystal growth. 1. 2. 3. 4.
E. Johnson, M. Aagesen, C.B. Sørensen, J. Nygård, P.E. Lindelof, Proc. 16th Int. Micr. Cong. Sapporo, Japan, (2006), p. 1168. A.I. Persson, M.W. Larsson, S. Stenström, B.J. Ohlsson, L. Samuelson, L.R. Wallenberg, Nature Materials, 3 (2004), p. 667. Z.H. Wu, X. Mei, D. Kim, M. Blumin, H.E. Ruda, J.Q. Liu, K.L. Kavanagh, Appl. Phys. Lett. 83 (2003), p. 3368. This work is supported by the Danish Natural Science Research Council.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 137–138, DOI: 10.1007/978-3-540-85226-1_69, © Springer-Verlag Berlin Heidelberg 2008
138
Figure 1. GaAs nanorods grown at 515 °C by MBE on a cleaved [100] GaAs wafer. The drawing shows the projection of the (112) directions on to the [011] plane of observation. The (112) rod indicated by arrow shows a typical morphology where one side is straight and smooth and the other side is wavy and rough. Only about 5% of the rods are of (112) type but they are about 10 times longer than other rods in the growth and therefore dominate the SEM image visually.
Figure 2. (112) GaAs nanorod. The bottom part with the straight edge has wurtzite structure with a (11-20) direction along the wire axis and the top part with the rougher edge has faulted and twinned zincblende structure with a (112) direction along the wire axis.
a)
5 nm b)
5 nm Figure 3. GaAs nanorods with wire axis along (11-20) in the wurtzite structure (a) and wire axis along (112) in the zincblende structure (b). Both structures contain faults, twins and lamellae of the opposite structure. Wire axes are vertical.
139
Structural characterization of ZnO nanorods grown on sapphire substrate by MOCVD P.-H. Jouneau1, M. Rosina2, G. Perillat1, 2, P. Ferret2 and G. Feuillet2 1. CEA - INAC, SP2M / LEMMA, 17 rue des Martyrs, 38048 Grenoble cedex 9, France 2. CEA - LETI, Minatec, 17 rue des Martyrs, 38048 Grenoble cedex 9, France pierre-henri.jouneau@cea fr Keywords: ZnO, nanowire, nanorod
ZnO is a promising material for light emitting devices at room temperature up to the ultraviolet spectral region thanks to a band gap of 3.37 eV and a large exciton binding energy (≈ 60 meV). The growth of defect-free material and the mastering of doping are however two requirements to fully exploit this potential. In this perspective, the fabrication of ZnO nanorods by catalyst-free metallorganic chemical vapour deposition (MOCVD) has recently attracted a large interest: the growth of vertical, well-aligned nanorods with uniform lengths and diameters, and without structural defects, has been reported, even if their formation is not yet well understood [1, 2]. In this study, the microstructure and the morphology of ZnO nanorods obtained without catalyst by MOCVD on (0001)-oriented sapphire have been investigated by SEM, HR-TEM and HR-STEM in an attempt to better understand the growth mechanisms. They are obtained for substrate temperatures of 750°C-850°C, using diethylzinc and N2O as precursors. Scanning electron microscopy revealed a high density of nanorods (up to 109 cm-2), aligned perpendicularly to the surface with a unique crystallographic orientation (Figure 1). The growth starts with a 2D monocrystalline layer, but of uneven thickness and with some porosity, followed by the formation of islands terminated by large hexagonal pyramids. Nanorods appear mostly at the top of these pyramids, with a hexagonal section (corresponding to a growth axis along the c-direction) and most often a facetted tip. Length, diameter and density vary with the growth time, reactor total pressure and N2O partial pressure, but each given sample present a high shape and size uniformity (with typical wires diameter of about 150 nm and length of about 4 μm). TEM gives more insight on the crystalline structure. Filtered convergent beam electron diffraction patterns along a <0 1 -1 0> axes and HR-STEM images reveal a Zn polarity of the nanorods, i.e. a growth direction corresponding to the [0001] direction. No structural defects are visible in the nanorods, but the analysis of defects existing in the underlying layer (dislocations and planar defects such as antiphase boundaries) allows us to give some insights on the possible growth mechanisms. 1. 2.
U. Özgur, Ya.I. Alivov, C. Liu, A. Teke, M.A. Reshchikov, S. Dogan, V. Avrutin, S.-J. Cho and H.Morkoç, J. Appl. Phys. 98 (2005) 041301 I.C. Robin, B. Gauron, P. Ferret, C. Tavares, G. Feuillet, Le Si Dang, B. Gayral and J.M. Gérard, Appl. Phys. Lett. 91 (2007) 143120.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 139–140, DOI: 10.1007/978-3-540-85226-1_70, © Springer-Verlag Berlin Heidelberg 2008
140
Figure 1. SEM images of ZnO nanorods vertically aligned on a (0001) sapphire substrate, showing uniformity in diameters and lengths. Nanorods grow on top of hexagonal pyramids, with a uniform crystallographic orientation, and most often a faceted summit.
Figure 2. STEM images of a nanorod showing no structural defects. Filtered <0 1 -1 0> CBED patterns taken at various distances from the centre evidence the Zn polarity of the nanorod when compared with simulated patterns.
141
Nucleation of Metal Clusters on Carbon Nanotubes X. Ke1, A. Felten2, D. Liang1, S. Bals1, J.J. Pireaux2, J. Ghijsen2, W. Drube3, M. Hecq4, C. Bittencourt4 and G. Van Tendeloo1 1. EMAT, University of Antwerp, Groenenborgerlaan 171, B-2020 Antwerp, Belgium 2. LISE, University of Namur, B-5000 Namur, Belgium 3. DESY, Hasylab, D-22603 Hamburg, Germany 4. LCIA, University of Mons-Hainaut, B-7000, Mons, Belgium [email protected] Keywords: Carbon Nanotubes, metal contact, chemical interaction
Electromigration in metal interconnects limits the number of devices in a single microprocessor. This limitation has already led to the replacement of Al as interconnect material by Cu, which has a higher current carrying capacity of the order of 106 A/cm2. Nevertheless, as the dimensions of the interconnect lines continue to shrink, electromigration and stress-induced migration phenomena remain reliability concerns for inlaid copper interconnects. CNT’s, capable of carrying currents of the order of 109 A/cm2, appear as a good candidate to replace state-of-the-art inlaid copper interconnects in microprocessors. A key step for integration of CNT’s in actual devices is the formation of stable and low-resistance ohmic contacts. Palladium appears as the most promising contact metal; elimination of the Schottky barrier and ballistic transmission of electrons has been already reported [1]. However, there is no obvious reason why Pd should give a smaller barrier than, say, Pt. Why is its electrical behaviour different? Does palladium react chemically with the CNT? Here we investigate the interaction between CNT’s and three different metals, namely platinum, palladium and gold, which are thermally evaporated onto CNT’s. High Resolution Transmission Electron Microscopy (HRTEM) was used to monitor the nucleation and evolution of the metal coatings on the CNT’s, whereas chemical interaction was monitored by X-ray photoemission spectroscopy (XPS). It was observed that during the onset of the evaporation, clusters are formed at the CNT surface (Figure 1). Electron tomography will be carried out to gain threedimensional information on how the CNT is coated with clusters. The cluster size increases by forming a quasi-continuous coating onto the CNT surface when the amount of metal evaporated on the surface is increased. Functionalization of the CNT surface leads to a better dispersion of the clusters and reduces the cluster size by creating more active sites for clusters to nucleate. Figure 2 shows a metal cluster on top of a CNT surface. The preserved structure of the graphene layers under the cluster suggests the absence of a mixed metal-carbon phase. Further information and confirmation can be obtained by XPS. If a chemical reaction is present at the interface, then the chemical environment of the atoms at the interface will show new features in the XPS spectra. The absence of new features near the metal core levels spectra (Figure 3) proves that no Pt-C, Pd-C or Au-C bonds are formed.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 141–142, DOI: 10.1007/978-3-540-85226-1_71, © Springer-Verlag Berlin Heidelberg 2008
142
The increase in the FWHM of the core-levels and the shift in the binding energy (Figure 3) will be discussed in terms of intrinsic initial electronic structure and final states effect.
Figure 1. TEM image of CNT’s coated with Pt. Au 4f
Intensity (arb. units)
Pt 4f
Intensity (arbt. units)
Intensity (arb. units)
Pd 3d
Figure 2. TEM image of CNT decorated with Pd clusters.
20 Å 10 Å 5Å 2Å 1Å 0.3 Å
350
345
340
335
Binding Energy (eV)
330
92
90
88
86
84
Binding Energy (eV)
82
80
80
78
76
74
72
70
68
66
Binding Energy (eV)
Figure 3. XPS spectra shows the evolution of the metal core levels by increasing amount of metal evaporated onto the CNT’s surface. 1. 2.
J. Tersoff Nature 23 (2003), p. 622 This work is supported by the Belgian Program on Interuniversity Attraction Pole (PAI 6/08) and by DESY and the European Commission under contract RII3-CT 2004-506008 (IASFS). JG is research associate of NFSR (Belgium).
143
EDX and linescan modelling for core/shell GaN/AlGaN nanowire analysis L. Lari1, R.T. Murray1, T. Bullough1 P.R. Chalker1, C. Chèze2, L. Geelhaar3 and H. Riechert 2 1. Department of Engineering, University of Liverpool, Liverpool, L69 3GH, UK 2. Paul-Drude-Institut für Festkörperelektronik, 10117 Berlin, Germany 3. Namlab, 01187 Dresden, Germany [email protected] Keywords: EDX, nanowires, GaN, AlGaN
The growth of gallium nitride nanowires (NW) using nickel seeds to promote axial growth on sapphire substrates has previously been demonstrated [1]. Furthermore it has been shown that control of preferential axial or radial growth can be achieved by changing the group III:V flux during growth using either N-rich or Ga-rich conditions respectively. The next challenge is controlled growth of NW heterostructures incorporating both GaN and AlGaN. This achievement would open the way to development of nanoelectronic devices such as single wire III-nitride based field effect transistors. A critical issue is the control of Al incorporation in GaN/AlGaN radial NW heterostructures. This study reports the Al distribution analysis in such radial nanowires heterostructures grown by plasma assisted Molecular Beam Epitaxy on c-sapphire. The sample consists of a GaN NW core initially grown under N-rich conditions followed by an Al0 2Ga0 8N “shell” grown under Ga-rich conditions. NWs have diameters typically between 20 and 100 nm and lengths of around 1-1.5 μm. Compositional analyses were made using energy dispersive X-ray analysis (EDX) in a VG HB601UX FEG-STEM operating at 100 KV and equipped with a windowless Si(Li) EDX spectrometer. EDX spectra from point analysis were quantified using thin film approximation with calculated K factors using both the Zaluzec and Mott-Massey models [2]. Line scans profiles were obtained integrating selected energy windows centered in the Al and Ga K lines peaks with an appropriated choice of windows for background removal from the raw profiles. EDX point analyses on the NWs show an aluminium concentration, in the radial shell, which decreases as you go from the NW growth tip towards the NW root end at the substrate (Figure 1). Elemental net intensities from transversal EDX line scans across the NWs are interpreted using a geometric model of the EDX excitation volume within the core and shell region assuming the NW cross-section to be either hexagonal or radial (Figure 2). The sensitivity of the model to the AlGaN shell thickness, as it changes along the NW length, is discussed as well with the implications on the growth mechanism for these NW structures in group III-rich condition.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 143–144, DOI: 10.1007/978-3-540-85226-1_72, © Springer-Verlag Berlin Heidelberg 2008
144
1. 2. 3.
L. Geelhaar, C. Chèze, W.M. Weber, R. Averbeck, H. Riechert, T. Kehagias, P. Komninou, G.P. Dimitrakopulos, and T. Karakostas, Appl. Phys. Lett. 91 (2007) 093113. D. C. Joy, A. D. Roming and J. I. Goldstein in “Principles of analytical electron microscopy” (Plenum Press, New York) (1986), p. 163. This work was supported by the EU contract MRTN-CT-2004-005583 (PARSEM) and the IST project NODE 015783.
(A)
(B)
Figure 1. (A) STEM bright field image of GaN/AlGaN core/Shell NW heterostructure. Results report Al at% from EDX point analysis quantification using Zaluzec (MottMassey) cross-section models. (B) Variation of Al at% across the NW diameter consistent with the core/shell structure
(nm)
(nm)
Figure 2. (A) STEM bright field image of a typical NW tip the arrow reporting the position of the line scan corresponding to the experimental profile in (C and D). (B) NW core shell structure obtained from the best fitting with both radial and hexagonal Xsection models. (C, D) EDX and modelled profiles assuming different shell thickness.
145
Mo6S9-xIx nanowires: structure studies by aberration corrected high resolution TEM and STEM V. Nicolosi1, J.N. Coleman2, D. Mihailovic3 and P. Nellist1 1. Department of Materials, University of Oxford, OX1 3PH, Oxford, UK 2. School of Physics, University of Dublin, Trinity College, D2, Dublin, Ireland 3. Josef Stefan Institute of Ljubljana, Jamova 39, 1000 Ljubljana, Slovenia [email protected] Keywords: nanowires, HRTEM, STEM
In the last few years carbon nanotubes have attracted a great deal of attention because of their interesting properties, including dependence of their chemical and electronic behaviour on their small dimension, high anisotropy and tube-like structure. Since nanotubes are difficult to process, one-dimensional inorganic nanowires have been receiving growing attention as a viable alternative to nanotubes. The most promising of these are the Mo6S9-xIx family. Easy fabrication [1], easy dispersability and processability [2], and uniformity in terms of metallic character [3] as well as diameter, makes Mo6S9-xIx nanowires one of the most promising one-dimensional materials. In order to fully understand their properties it is imperative to confirm the atomic structure of those mono-dimensional objects. Here we present a combined aberration corrected high resolution transmission electron microscopy (HRTEM) and scanning transmission electron microscopy (STEM) study of Mo6S9-xIx nanowires. Annular dark-field (ADF) STEM allows imaging of the individual one-dimensional molecules that aggregate to form bundles (Figure 1), but is unable to image the lower atomic number S atoms. Phase contrast HRTEM is less sensitive to Z, and reveals complementary information. Electron microscopy, crystallographic and electron microscopy-simulated studies allow us to determine both the unit cell structure and the packing structure of the wires in the bundles. Studies on Individual Mo6S3I6 nanowires can be best described as one-dimensional molybdenumchalcogenide-halide clusters. Mo-octahedra appear surrounded by iodine atoms and connected by bridging planes of three sulfur atoms (Figure 2). The nanowires tend to be weakly bounded into bundles by van der Waals forces, in a triclinic lattice arrangement, with a nanowire to nanowire distance of 0.958nm [3]. Data for other nanowire stoichiometries, such as Mo6S4 5I4 5 and Mo6S2I8, will be also presented. 1. 2. 3.
D. Vrbanic, M. Remskar, A. Jesih, A. Mrzel; P. Umek, M. Ponikvar, B. Jancar, A. Meden, B. Novosel, S. Pejovnik, P. Venturini, J. N. Coleman, D. Mihailovic, Nanotechnology 15 (2004), 635-638. V. Nicolosi, D. Vrbanic, A. Mrzel, J. McCauley, S. O’Flaherty, D. Mihailovic, W. J. Blau, J. N. Coleman, Journal of Physical Chemistry B, 109 (2005), 7124-7133 V. Nicolosi, P. D Nellist, S. Sanvito, E. C. Cosgriff, S. Krishnamurthy, W. J. Blau, M. L. H. Green, D. Vengust, D. Dvorsek, D. Mihailovic, G. Compagnini, J. Sloan, V. Stolojan, J. D Carey, S. J Pennycook, J. N. Coleman, Advanced Materials, 19, 4, (2006) 543-547
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 145–146, DOI: 10.1007/978-3-540-85226-1_73, © Springer-Verlag Berlin Heidelberg 2008
146
Figure 1. Typical Annular Dark Field STEM image of a MoSI nanowire bundle. The coexistence of four different patterns can be explained by the fact that, seeing that those systems possess very low sheer modulus, a twisting process along the longitudinal axis of the same nanowire bundle is very likely to happen. This therefore produces different projections. Image taken using a using a VG HB501 instrument fitted with a Nion Cs corrector.
Figure 2. Structure of a Mo6S3I6 nanowire. Red, purple and yellow represent in order molybdenum, iodine and sulfur atoms. The brackets define the nanowire unit cell.
147
Discrete Atom Imaging in Carbon Nanotubes and Peapods Using Cs-Corrected TEM Operated at 100keV Luca Ortolani1,2,3, Florent Houdellier3,Marc Monthioux3 1. CNR-IMM Bologna, v. Gobetti, 101, 40129 Bologna, Italy 2. Physics Dept., University of Bologna, v.le B. Pichat 6/2, 40127 Bologna, Italy. 3. CNRS CEMES, 29, rue Jeanne Marvig, 31055 Toulouse [email protected] Keywords: Cs Corrected TEM, Peapods, Carbon Nanotubes
The filling of carbon nanotubes (CNTs) with inorganic crystal as well as organic molecules or fullerenes has been widely investigated over the last years [1]. Filled Multi-Walled CNTs and, first of all, Single-Walled CNTs have become the most promising hybrid-nanomaterials for many applications because of the strong interaction between the outer carbon shell and the inner material and the imposed 1D dimension, capable to modify the atomic structure of both the filling and the nanotube [2]. Structural characterization by TEM is hampered by SWCNTs very small dimension and by its relative instability under the electron beam. Notwithstanding the outer carbon shell may act as a protecting environment, allowing the observation of the structure and of the dynamic behaviour of the contained molecules, in conventional 200 keV imaging, beam electrons are capable of displacing carbon atoms from the graphene lattice, resulting in a rapid destruction of the tube. Moreover, in conventional TEM observations of filled SWCNTs, the nanotubes themselves have been regarded as almost contrast-less container materials, due to the limited spatial resolution [3,4]. The use of aberration-corrected TEMs and lower observation energies seems to be the most promising experimental approach to study this kind of materials. We report here the results obtained on carbon structures and radiation-sensitive materials with the SACTEM-Toulouse, a TECNAI F20 equipped with a spherical aberration (Cs) corrector that was able to be operated at 100kV, for the first time we believe. The new lens set-up allows easy imaging of CNTs, as can be seen in Figure 1a. The Cs, and all the aberrations up to the fourth order, has been completely removed, and the graphene lattice of the CNT can be resolved. Moreover, the corrector is capable also to set the spherical aberration to a specified negative value in order to compensate the residual resolution-limiting aberration, which is, in our set-up, the 8 mm fifth-order spherical aberration. Therefore, a negative Cs of -19 μm can be used to compensate for this aberration, the same way defocus can be used to compensate Cs [5,6], resulting in a clearer resolution of fullerenes structure, as shown in Figure 1b. An interesting feature of Cs-corrected TEM is that a small change in focus affects dramatically the contrast of different z-planes in the specimen [3]. This effect is evident in the focus series of Figure 2: in a) and c) the contrast of the contained fullerenes is enhanced; in b), the contrast of the graphene lattice is maximized, while fullerenes have almost disappeared.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 147–148, DOI: 10.1007/978-3-540-85226-1_74, © Springer-Verlag Berlin Heidelberg 2008
148
1. 2. 3. 4. 5. 6.
M. Monthioux, Carbon 40 (2002), p. 1809. J. Sloan et al., Acc. Chem. Res. 35 (2002), p. 1054. K. Hirahara et al., Nano Lett. 6 (2006) p. 1778 Y. Sato et al., Nano Lett. 7 (2007), p. 3704. O. Scherzer, J. Appl. Phys. 20 (1949), p. 20. S. Uhlehmann, M. Haider, Ultramicroscopy 72 (1998), p. 109.
Figure 1. a) Image of a SWCNT, using Cs=0. Graphene lattice is clearly resolved. b) Image of a peapod, Cs=-19μm.
Figure 2. Focus series of a peapod (Cs=0). Focussing is decreasing from a) (overfocus) to c) (underfocus).
149
Extended Defects in Semiconductor Nanowires Peter Pongratz1, Youn-Joo Hyun2, Alois Lugstein2, Aaron Andrews2 and Emmerich Bertagnolli2 1. Institute of Solid State Physics,TU-Wien, Wiedner Hauptstrasse 8-10, A-1040 Vienna, Austria 2. Institute of Solid State Electronics, TU Wien, Floragasse 7, A-1040 Vienna , Austria [email protected] Keywords: nanowires, TEM analysis, extended defects
Epitaxial growth of semiconductor nanostructures has opened new frontiers in semiconductor physics. Silicon and various other III-V semiconductor nanostructures grown on silicon wafers with various orientations and under different growth conditions have been successfully demonstrated by many groups [1,2,3]. TEM and electron diffraction techniques which are able to analyse these whiskers in detail have shown that even unconventional hexagonal structures of Si, GaAs and Ge could be generated under these conditions. We have studied these nanowires changing nucleation and growth conditions ( e.g. gas fluences or pressures, temperatures etc.) and found not only perfect single crystalline structures but also extended defects such as dislocations, stacking faults, twins, and grain boundary and interface structures. Using TEM analysis and refined cross-section preparation techniques they can be seen along the whiskers which are related to these growth conditions [4]. It is clear that it is essential to understand the relations between defects and growth conditions if a perfect control of the nanostructure growth process is desired. It is clear that not only the growth directions are of importance but also the structure of the side walls, the nucleation conditions at the substrate and the wetting conditions at the catalyst particles’ interface in the case of VLS growth . We will present our results related to the branching of nanowire trees on a trunk of silicon or the regularity of the cross-sections in the case of heteroepitaxial tree-structures. We have analysed kinks, dislocations and microtwins related to changing growth conditions but also complicated stacking faults and facets related to anisotropy effects and variable surface orientations . Elastic strains and surface energies are certainly more important for the properties of these nanowires than for their extended three dimensional counterparts. We will present various examples how HRTEM electron microscopy and analysis are extremely valuable to find out these details on a nanometer scale.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 149–150, DOI: 10.1007/978-3-540-85226-1_75, © Springer-Verlag Berlin Heidelberg 2008
150
a
0.326 nm
b
Figure 1 (a) Cross sectional TEM and HRTEM image of a GaAs whisker and the respective SAED pattern recorded along the nanowhisker axis. (b) HRTEM image of the GaAs whisker with the GaAs whisker tip in the inset. 1. 2. 3. 4. 5.
T.Martenson ,C. Svensson , B Wacaser et al. Nano Lett. 4 (1987) Björk,M, B. Ohlsson T. Sass , A. Persson et al. Nano Lett. 2, 87 (2002) H. Jagannathan, M. Deal, Y. Nishi et.al. J.Appl. Phys.100, 024318 (2006) A. Lugstein A Andrews, M. Steinmair, Y. Hyun et al. Nanotechnology 18, 355306 (2007) We kindly acknowledge support by Austrian Science Fund P-18080-N07; Sixth EU Framework (NoE) SANDiE ; TU Vienna-USTEM and Austrian Society for Micro and Nanoelectronics
151
Surface chemistry along a single silicon nanowire: Quantitative x-ray photoelectron emission microscopy (XPEEM) of the metal catalyst diffusion O. Renault, A. Bailly, P. Gentile, N. Pauc, T. Baron, L.–F. Zagonel, N. Barrett 1. CEA-LETI, MINATEC, 17, rue des Martyrs, 38054 Grenoble Cedex 09, France. 2. CEA-DSM/INAC/SP2M/SiNaPS, 17 rue des Martyrs, 38054 Grenoble cedex 9, France. 3. Laboratoire des Technologies de la Microélectronique, UMR CNRS 5129, 17 rue des Martyrs, 38054 Grenoble cedex 9, France. 4. CEA-DSM/IRAMIS/SPCSI, CEA Saclay, 91191 Gif-sur-Yvette, France. [email protected] Keywords: silicon, nanowire, diffusion, XPEEM, threshold photoemission.
Understanding and controlling the growth, usually performed by Vapour-LiquidSolid method, of silicon nanowires with grown metal catalysts is crucial for optimized morphologies, surface and electronic properties of these nanostructures regarding their future applications. One of the issues is the suppression of the tapering effect resulting in a cone-shaped wire, and arising from the diffusion, during growth, of the metal catalyst along the sidewall. Indirect evidences for such a phenomenon and for the presence of gold on the sidewall have been proposed previously [1], before a qualitative and direct identification using SEM-EDX and TEM was reported for technologically relevant Si NWs [2]. However, such techniques cannot provide quantitative and surfacesensitive information relevant to the diffusion process, and moreover can be extremely localized, preventing to obtain a global picture of the surface chemistry at the scale of the wire. For the first time, we quantify at a mesoscopic scale the surface chemistry of single, tapered silicon nanowire (100-250 nm diameter), using a novel X-ray photoelectron emission microscopy (XPEEM) with aberration-corrected energy-filtering and soft xray synchrotron illumination (ID08 beamline, ESRF) [3]. This spectromicroscope enables full-field, energy-filtered imaging using either secondary or core-level photoelectrons, giving information respectively about the local work function or the chemical state of the considered elements [4]. With XPEEM we provide a direct, nondestructive chemical confirmation of gold migration along the sidewall surface from threshold and core-level photoemission localized nanospectra. In particular, the secondary electron nanospectra, generated over a typical 200x200 nm2 area at the photoemission threshold from the images shown in Figure 1, have a remarkable doublestructure indicative of two distinct chemical phases present at the surface; the work function of which can be retrieved by modeling using Henke’s functions [3]. The values of work-functions Φ1 and Φ2, close to 4.1 and 5.0 eV, respectively, are in agreement with reported values for silicon nanowires and gold. The presence of gold all along the sidewall is further confirmed with the Au4f7/2 core-level image and corresponding
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 151–152, DOI: 10.1007/978-3-540-85226-1_76, © Springer-Verlag Berlin Heidelberg 2008
152
nanospectra (Figure 2). From the Au4f7/2 and Si 2p core-level local intensities weighed by the corresponding photoionization cross-sections, we have access to the partial coverage, θAu, of gold on the nanowire sidewall. Gold has an evenly distributed island structure, covering 0.42 ± 0.06 of the nanowire surface corresponding to ~1.8 ML, in full agreement with independent transmission electron microscopy results. 1. 2. 3. 4. 5.
J. B. Hannon, S. Kodamka, F. M. Ross and R. M. Tromp, Nature 440, 69-71 (20006). F. Dhalluin et al., J. Appl. Phys. 102, 094906 (2007). A. Bailly, O. Renault et al., Phys. Rev. Lett., submitted. M. Escher et al., J. Phys. : Cond. Matter 17, S1329 (2005). This work was carried out with the financial support of the French ANR “XPEEM” project 05-NANO-065-02. Special thanks go to the staff of the ID08 beamline at the ESRF for their technical help during the experiments.
Figure 1. Energy-filtered XPEEM images at the photoemission threshold (workfunction contrast) and nanospectra on the sidewall (I, II), the catalyst (III) and the gold substrate (IV). Contrast inversion occurs when the electron energy exceeds the work function of the gold substrate (5.1 eV). Φ1 and Φ2 correspond to the first and second photoemission threshold, respectively at low and high energy.
Figure 2. XPEEM Au4f7/2 core-level image (left) and nanospectra (center). Right : Gold coverage derived from the Au4f and Si 2p local core-level intensities. Schematic drawing of the main corridors through which automobilists can reach the Eurogress Centre. Drawing is not to scale.
153
TEM characterization of metallic Ni nanoshells grown on gold nanorods and on carbon nanotubes J.B. Rodríguez-González, M. Grzelczak, M.A. Correa-Duarte, J. Pérez-Juste and L.M. Liz-Marzán Departamento de Química Física, Unidad Asociada CSIC-Universidade de Vigo, 36310 Vigo, Spain. [email protected] Keywords: TEM, nickel, shells.
Anisotropic, magnetic nickel shells were grown on gold nanorods [1] and on carbon nanotubes (CNT) [2] using Pt nanocrystals as catalysts. We used high resolution transmission electron microscopy (HRTEM) to characterize these well-defined metallic nickel shells. In gold nanorods, Pt nanocrystals were selectively grown on the nanorod tips [3], and Ni2+ was subsequently reduced over them, in a quasi-epitaxial growth demonstrated by HRTEM and electron diffraction. Figure 1a shows a distinct contrast between the darker gold core and the lighter Ni shell, with a high degree of roughness in the shell, which might indicate the presence of an outer, thin NiO shell. The area corresponding to the gold core is almost completely covered with Moiré fringes arising from the presence of two superimposed different crystalline lattices in a quasi-epitaxial growth, confirmed by nanobeam diffraction (NBD). The distribution of Au and Ni within the particles was also investigated by scanning transmission electron microscopy STEM-XEDS elemental mapping (Figure 1b). A detailed analysis of the interface between gold core and nickel shell (Figure 1c and 1d) shows the presence of dislocations in this interface. TEM images of the CNT/Pt@Ni samples (Figure 2a) evidence the homogenous coating of individual CNTs and reveal the polycrystalline nature of the Ni layer on the final magnetic nanowires (Figure 2b). STEM-XEDS elemental mapping (Figure 2c) show the relative distribution of the elements; clearly Pt is located in the inner side of the metallic shell while Ni is mostly covering the outer part, as expected for an onionlike structure. HRTEM and SAED analysis also confirm the presence of unchanged CNTs in the inside part. 1. 2. 3.
M. Grzelczak, B. Rodríguez-González, J. Pérez-Juste, and L. M. Liz-Marzán, Adv. Mater. 19 (2007), 2262. M. Grzelczak, M. A. Correa-Duarte, V. Salgueiriño-Maceira, B. Rodríguez-González, J. Rivas, and L. M. Liz-Marzán, Angew. Chem. Int. Ed. 46 (2007), 7026. M. Grzelczak, J. Pérez-Juste, B. Rodríguez-González and L.M. Liz-Marzán, J. Mater. Chem. 16 (2006), 3946.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 153–154, DOI: 10.1007/978-3-540-85226-1_77, © Springer-Verlag Berlin Heidelberg 2008
154
Figure 1. Nickel coated gold nanorods. a) Note the presence of Moiré fringes and the shell roughness. b) STEM-XEDS elemental mapping. c) Interface between gold core and nickel shell. d) FFT filtering of (c).
Figure 2. Nickel coated carbon nanotube. a) Bright field image of one CNT/Pt@Ni. b) Outer Ni layer. c) STEM-XEDS elemental mapping.
155
Electron Irradiation Effects in Carbon Nanostructures: Surface Reconstruction, Extreme Compression, Nanotube Growth and Morphology Manipulation M. Terrones1, L. Sun2, J.A. Rodriguez-Manzo3, H. Terrones1, and F. Banhart3 1. Advanced Materials Department, IPICyT, 78216 San Luis Potosí, México 2. Institut für Physikalische Chemie, Universität Mainz, D-55099 Mainz, Germany 3. Institut de Physique et Chimie des Matériaux, UMR 7504, F-67034 Strasbourg [email protected],mx Keywords: electron irradiation, nanotube growth, extreme compression
It will be demonstrated, that irradiation exposure at elevated temperatures, can be used as an effective tool to covalently weld SWNTs in order to create molecular junctions of various geometries [1-3]. We have fabricated Y, X and T-like junctions that are stable [2]. Tight binding molecular dynamics calculations demonstrate that vacancies, formed under the electron beam, trigger the formation of molecular junctions involving seven or eight membered carbon rings. We envisage that these results will pave the way towards controlled fabrication of novel nanotube-based molecular circuits, nanotube fabrics and network architectures. In this context, novel super architectures, using carbon nanotubes as building blocks will be discussed, and their mechanical and electronic properties presented, as well as their possible applications [4]. We will also show that the melting and solidification behavior of metal crystals can be drastically altered when they are encapsulated in fullerene-like graphitic shells [5]. The melting temperature of low melting point metal crystals (e.g. Bi, Sn, Pb, etc.) inside graphitic shells is increased relative to the bulk melting point by a much larger amount than that observed for metal crystals embedded in other materials. It appears that graphite is the ultimate material for enhancing the melting/solidification hysteresis of small crystals or clusters. Therefore, metal clusters encapsulated by graphitic shells may be potentially advantageous in temperature-resistant crystalline composite materials. In addition, we will demonstrate that controlled irradiation of MWNTs can cause large pressure buildup within the nanotube cores, to the extent of being able to plastically deform, extrude, and break solid materials that are encapsulated inside [6]. We further show by atomistic simulations that the internal pressure inside nanotubes can reach values higher than 40 GPa. Nanotubes can thus be used as robust nanoscale jigs for extruding hard nanomaterials and modifying their properties, as well as templates for other highpressure applications at the nanoscale. Finally, it was observed that when MWNTs containing metal particle cores are electron irradiated, carbon from graphitic shells surrounding the metal particles is ingested into the body of the particle and subsequently emerges as single- or multi-walled nanotubes inside the host nanotubes. These observations at atomic resolution in an electron microscope and indicate that bulk diffusion of carbon through the body of catalytic particles is the growth-limiting process [7].
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 155–156, DOI: 10.1007/978-3-540-85226-1_78, © Springer-Verlag Berlin Heidelberg 2008
156
1. 2. 3. 4. 5. 6. 7.
M. Terrones, et al. Science 288 (2000), 1226. F. Banhart, et al. Small 1 (2005), 953. M. Terrones, et al. Phys. Rev. Lett. 89 (2002), 075505. J.M. Romo-Herrera, et al. Nano Letters 7, (2007), 570. F. Banhart, F., et al. Phys. Rev. Lett. 90 (2003), 185502. L. Sun, et al. Science 312 (2006), 1199. J.A. Rodríguez-Manzo, et al. Nature Nanotechnology 2 (2007), 307.
Figure 1. SWNT growth from a Co crystal. The growth happens under electron irradiation (intensity 100 A cm-2) at a specimen temperature of 600 °C. a) Image before growth; b) Image after 345 s of irradiation: and c) Image after 475 s.
Figure 2. (a-c) HRTEM images of a “T-like” junction formed after irradiating a “Y” junction. It is possible to thin one of the tubes of the “Y” junction, which eventually breaks and forms a “hook” (not shown here). It is also possible to observe the evolution of this junction during irradiation and the rotation by 180° under the electron beam; note the circular cross-section in one of the tubes (b).
157
Crystallographic phase and orientation analysis of GaAs nanowires by ESEM, EDS, TEM, HRTEM and SAED A.M. Tonejc1, S. Gradečak2, A. Tonejc1 , M. Bijelić1, H. Posilović3, V. Bermanec3 and M. Tambe 2 1. Faculty of Science, Dept. of Physics, Bijenička 32, 10002 Zagreb, Croatia 2. MIT, Dept. Mat. Sci. Engng., 77 Massachusetts Avenue, MA02139 Cambridge, USA 3. Faculty of Science, Dept. of Geology, Horvatovac 102, 10002 Zagreb, Croatia [email protected] Keywords: GaAs nanowires, ESEM, TEM/SAED
The novel properties of semiconductor nanowires are interesting [1] for application and could be useful for application in nanoelectronics and photonics. Depending on the band gap and size of particular semiconductor nanowires, the shift in absorption/emission is observed. The samples were grown by general synthetic method developed by the C.M. Lieber group [2]. The method controls both the diameter and the length of nanowires (NW) during growth. This approach uses monodisperse nanocluster catalysts Au to define both the nanowire diameter and initiation of nanowire elongation during growth by a vapour–liquid-solid mechanism. In this article, as prepared GaAs NW samples, grown on GaAs [100] and [111] oriented films were synthesized using gold nanocluster catalyst and metalorganic chemical vapour deposition. Figure 1a shows ESEM photographs of NW vertically grown on GaAs [111] oriented film. It is the region from the edge of the sample to measure distribution of the NW lengths (Figure 1b) and the distribution of catalytic gold particles displayed in Figure 1c. The diameter of the catalytic particles at the top of the NW of diameter is (94±20) nm, that had to be the same as NW diameter. Belonging EDS spectrum (Figure 1d) shows the presence of Ga, As and Au. Figure 2a shows NW of GaAs observed by ESEM and EDS grown on [111] films. In Figure 2c TEM image of NW having diameter d= (32 ±10) nm, measured from TEM, is shown. The corresponding SAED in [111] Au orientation of the catalytic particles shows as well as HCP the {001} GaAs spots. The SAED (Figure 2d) gives evidence that the substrate film had the same orientation. The growth direction of NW is [011] and the structure is identified as HCP GaAs, according to ICDD-PDF No. 80-0003. The distribution of the lengths of nanowires is given from 500 to 3500 nm with maximum values 1300 and 2000 nm, for two observed samples, Figure 1c and Figure 2b, respectively. From HRTEM images it is found that NWs are coated with 3 to 5 nm thick amorphous layer. 1. 2.
M. Law, J. Goldberg and P. Yang, Annu. Rev. Mater. Res. 34 (2004), p. 83. Y. Cui, L.J. Lauhon, M.S. Gudiksen, J. Wang and C.M. Lieber, Applied Physics Letters 78 (2001), p. 2214.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 157–158, DOI: 10.1007/978-3-540-85226-1_79, © Springer-Verlag Berlin Heidelberg 2008
158 V a ri a b l e : V a r2 D i s t ri b u t i o n : L o g -n o rm a l
(a)
C h i -S q u a re t es t = 4 5 7 2 5 2 d f = 4 (a d ju s t e d )
p = 0 33 4 0 3
20
(b)
18 16 14 12 10 8 6 4 2 0
29 0909 58 1818 87 2727 116 3636 145 4545 174 5455 43 6364 72 7273 101 8182 1 30 9 0 9 1 160 0000 189 0909 C t
(d)
(
li
it )
Va ria b l e Va r2 , Di s tri b u ti o n L o g -n o rm a l Ch i -Sq u a re te s t
5 ,6 0 5 0 4, d f
2 (a d j u s te d ) , p
0 ,0 6 0 6 6
16
(c)
14 12 10 8 6 4
kV
1μm
2 0
520
1 0 40 780
1 5 60 1 3 00
2080 1 8 20
2 6 00 2340
3 1 20 2 8 60
Figure 1. Sample 1: (a) ESEM analyses of [111] grown GaAs NWs, the edge region; (b) The distribution of Au catalytic particles on the top of the NW; (c) The distribution of NW lengths; (d) EDS spectrum.
(c)
Vari a b e : Va 2 , Di s t i b uti o n : L o g -n o rm a l Ch i -Sq u a re te s t = 1 ,0 3 6 8 3 , df = 2 (ad j us te d ) , p = 0 ,5 95 6
(b)
18 16 1
(d)
(022)
12
(202)
10 8 6
(022)
2 0
5 0 0 10 0 0 1 5 0 0 20 0 0 2 5 0 0 30 0 0 3 5 0 0
000
5 0 0 50 0 0 5 5 0 0
[111]
1μm
(100)
(a)
(202)
50nm
Figure 2. Sample 2: (a) ESEM; (b) The distribution of the lengths measured by ESEM; (c) TEM measurements; (d) SAED in [111] Au orientation gives direction of the NW growth in the image (c).
159
3-Dimensional Morphology of GaP-GaAs nanowires M.A. Verheijen1, R. Algra2, M.T. Borgström1, G. Immink1, E. Sourty4, L.F. Feiner1, W.J.P. van Enckevort 3, E. Vlieg3 and E.P.A.M. Bakkers2 1. Philips Research, High Tech Campus 11, 5656AE Eindhoven, the Netherlands 2. Nederlands Institute for Material Research (NIMR), 2628CD Delft, The Netherlands 3. Radboud University Nijmegen, Toernooiveld 1, 6525ED Nijmegen, The Netherlands 4. FEI Company, Achtseweg Noord 5, AAE, 5600 KA Eindhoven, the Netherlands [email protected] Keywords: nanowires, tomography, morphology
Semiconductor nanowires are promising candidates for enabling integration of new functionalities. based on the advantageous properties of III-V semiconductors, such as high carrier mobility and optical activity into existing silicon technology. Because of the small dimensions and the consequently large ratio of surface to bulk atoms, the nanowire surface morphology and resulting chemistry can considerably affect the nanowire (opto-) electronic properties, such as carrier mobility and luminescence quantum yield. An elegant way to suppress such surface related effects is to cap the wires with a wide bandgap material to form core/shell nanowire structures. So far, only the vapour-liquid-solid (VLS), i.e. the axial growth mechanism and the zinc blende crystal structure has been considered in relation to the of III-V nanowire side faceting. In order to design and optimise nanowire properties for optical, electrical or mechanical performance, it is essential to take control over the nanowire surface morphology by fully understanding the parameters affecting radial growth. We have investigated the morphology of heterostructured GaP-GaAs nanowires grown by metal-organic vapor phase epitaxy as a function of growth temperature and V/III precursor ratio. The vertical growth of these wires is accompanied by lateral growth (i.e. thickening of the nanowires). The ratio vertical-to-lateral growth is strongly dependent on the growth parameters. The study of heterostructured core-shell nanowires with transmission electron microscopy (TEM) tomography (Figure 1) allowed to resolve the three-dimensional morphology, and to discriminate between the effect of axial (core) and radial (shell) growth on the morphology. Combining tomography with HRTEM (Figure 3), SEM and HAADF, a temperature and precursor dependent structure diagram (Figure 2a) for the GaP nanowire core morphology was constituted, and the evolution of the different types of side facets during GaAs and GaP shell growth was characterised. An additional parameter determining the sidewall morphology is the density of stacking faults (SF). In low SF-density <111> grown wires, the most stable sidewall morphology is allowed to form, contrary to high SF-density <111> grown wires. STEM/HAADF and SEM imaging was used to characterise this sidewall morphology (Figure 2b,c).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 159–160, DOI: 10.1007/978-3-540-85226-1_80, © Springer-Verlag Berlin Heidelberg 2008
160
Figure 1. 3-dimensional reconstruction of the morphology of the bottom part of a GaPGaAs heterostuctured nanowire (obtained using STEM/HAADF tomography). 2’’
a
b
1
2
3
c
V/III
2’
1
2
3
Temperature
ZB WZ
Figure 2a: Schematic 3D representation of the various VLS GaP core morphologies. Morphology types 1, 2’’, 2, 2’ represent zincblende crystal structures, while type 3 shows the morphology of alternating zincblende (ZB) and wurtzite (WZ) segments in high temperature grown wires. HAADF image of low SF-density nanowire (b) and a transition area from low to high SF-density (c).
ZB
WZ
5 nm
Figure 3: High resolution TEM image of the various facets of ZB and WZ segments in a high temperature grown GaP nanowire.
161
Characteristics of Indium-Catalyzed Si Nanowires Z.W. Wang1, Z.Y. Li1 and F. Iacopi2 1. Nanoscale Physics Research Laboratory, School of Physics and Astronomy, University of Birmingham, Birmingham B15 2TT, UK. 2. IMEC, Kapeldreef 75, B-3001 Leuven, Belgium [email protected] Keywords: Si nanowire, indium, structure
Si nanowires are promising candidates for applications in nanoelectronics, opoelectronics, and sensors. Au is a highly efficient catalyst that is widely used in the growth of Si nanowires by the well-known vapor-liquid-solid growth mechanism. However, the mid-gap trap states in Si introduced by surface or bulk diffusion of Au can be a strong killer to minor carrier lifetime, thus limit the use of Au-catalyzed nanowires in Si-based technology industry [1,2]. Efforts have been made in searching for alternative catalysts. Recently, we have successfully acquired Si nanowires with high yield using indium nanoparticles as catalysts by plasma-enhancement [3]. Any potential applications of this type of nanowires into Si-based industry require systematic characterization of structure of the nanowires and deep understanding of their growth mechanisms. Here we report a detailed investigation of morphology and crystalline structure of the In-Si nanowries using high resolution transmission electron microscopy. The results will be compared with the Au-catalyzed nanowires. The Si-nanowires under investigation are synthesized using In nanoparticles with size range of 10 to 200 nm. Figure 1 (a) and (c) show that the droplet at the nanowire tip display spherical shape. The large contact angle to the Si nanowire can be attributed to the lower solubility of Si in indium than in gold. All wires show a base-to-droplet tapering characteristics. It is found that the tapering tendency depends strongly on the size of In droplets: the smaller the droplet, the larger the tapering. Statistical analysis shows that there is an approximate 2:1 ratio of the diameter of In-droplet to the wire diameter at the thin end. The growth orientation of the nanowires is also depending on the size of the droplet. The large droplets prevail in growth along the [111] direction. An example is given in Figure.1 (a) and (b), where the droplet diameter is 105 nm and the wire diameter is 47 nm at the thin end. The growth orientation changes from [111] to [110], as the size of the droplet decreases to around 60 nm. A typical example is given in Figure.1. (c) and (d) for the wire with the droplet size of 62 nm and the thin end wire diameter of 32 nm. The change of Si nanowires growth direction has been reported previously for Au-catalyzed Si nanowires. However, the crossover of growth orientation on Au-catalyzed Si nanowires is smaller, which is usually below 20 nm [4]. The difference may be attributed to the characteristic morphology of Si nanowire grown by using different catalysts. Indium has different surface energy and eutectic compositions as to Au, which may shift the growth-direction transition point. Twins are often observed in the nanowires. The inset in Figure.1 (b) displays the diffraction pattern from {111} twins, showing clearly this nanowire twins on both
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 161–162, DOI: 10.1007/978-3-540-85226-1_81, © Springer-Verlag Berlin Heidelberg 2008
162
{111} planes (see the markers A and B). The dislocation in the nanowires is not common, except at either the sidewall of the wires or the interface between the droplet and the wire. One of such dislocation is shown in Figure.1 (d) in a twin-free nanowire. In summary, our work suggests that, through fine control of the size of Innanoparticle catalysts, it is possible to control the morphology and growth orientation of the Si nanowires. 1. 2. 3. 4.
J. B. Hannon, S. Kodambaka, F. M. Ross, R. M. Tromp, Nature 440 (2006) 69. J.E. Allen, E.R. Hemesath, D.E. Perea, J. L. Lensch-Falk, Z.Y. Li, F. Yin, M.H. Gass, P. Wang, A.L. Bleloch, R.E. Palmer, L.J. Lauhonn, Nature Nanotechnology, online 10 Feb 2008 F. Iacopi, P.M. Vereecken, M. Schaekers, M. Caymax, N. Moelans, B. Blanpain, O. Richard, C. Detavernier, H. Griffiths, Nanotechnology 18 (2007) 1. Y. Wu, Y. Cui, L. Huynh, C.J. Barrelet, D.C. Bell, C. Lieber, Nano Letters 4 (2004) 433.
-11-1
200 11-1
-1-11
A
-200 1-11
`
(a)
800nm
B
(b)
20nm
20-2 0-22
-220 02-2
2-20 -202
(c)
800nm
(d)
4nm
Figure 1. TEM characterization of In-catalyzed Si nanowires. (a) A nanowire with its droplet size of 105 nm. (b) A magnified view of the marked area in (a) and SAED pattern (insert). (c) A nanowire with its droplet diameter of 62 nm. (d) A magnified view of the marked area in (c), SAED pattern (left) and one-dimensional FFT filtered image corresponding to the top right area in (d).
163
HRTEM contribution to the study of extraterrestrial nanocarbons and some earth materials analogues J.N. Rouzaud1 and C. Le Guillou1 1. Laboratoire de Géologie de L’Ecole Normale Supérieure, UMR 8538, Paris, France [email protected] fr Keywords: carbon nanoparticles, extraterrestrial carbon, earth analogues
Most forms of natural and anthropic terrestrial carbons can be found in the extraterrestrial carbons, and especially disordered carbons, graphite, nanodiamonds, onions, … They are often found as nanoparticles and will be named here ‘nanocarbons’. Primitive meteorites contain organic matter of unknown origin (similar to the terrestrial kerogens), and submitted to low temperature metamorphism, but also nanodiamonds and graphitized particles. Meteorites processed at high temperature (1000°C) gather graphitic carbons, stricto sensu graphite, and (nano)diamonds. Thus, meteorites frequently show surprising associations of carbon phases usually synthesized in very different conditions of temperature and pressure [1]. To explain such paradoxical associations, different steps of meteorite processing must be involved (condensation of the protosolar gas, accretion, metamorphism on the parent-body, differentiation, shocks, …) and blends of different components are frequently put forward. To better understand the carbon components formation in Nature, our approach is to compare these natural carbons with possible synthetic earth materials analogues, obtained in well constrained conditions. The aim is to simulate the processes to which carbonaceous matter could have been submitted during their History in space. So, studies were performed on nanocarbons formed by different processes : pyrolysis with or without high pressures, laser pyrolysis, detonation, shocks, chemical vapour deposition, iron catalysed graphitization … The multiscale organisation of these natural and synthetic nanocarbons was studied by High Resolution Transmission Electron Microscopy (HRTEM) with a special interest for the nanometre scale. For disordered carbons, an original image analysis was developed to obtain more quantitative structural data [2]. Some examples of possible earth analogues will be presented: formation of nanodiamond from graphite heated at 1500°C under 15 GPa (Figure 1a from [3], graphitisation of detonation nanodiamonds (Figure 1b). Our approach will be especially illustrated by the comparison between the carbons found in an ureilite (enigmatic thermally processed meteorite) and those obtained by a ‘simple’ shock loading on pure graphite. Ureilites are characterized by a rather paradoxal association of diamond, lonsdaleite, graphite and disordered carbons. Possible synthetic analogues were obtained by 40 GPa, shock loading experiments on graphite [4]. At the nanometre scale, carbon associations are strikingly similar to ureilite carbons. Both natural and analogues samples contain more or less ‘distorted’ graphite grains and nanodiamonds, surrounded by disordered carbon (Figure 2a). The meteorite carbon also shows distorted graphite particles with diamond inclusions (Figure 2b). The
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 163–164, DOI: 10.1007/978-3-540-85226-1_82, © Springer-Verlag Berlin Heidelberg 2008
164
remarkable parallel contacts between 111 diamond planes and the 002 graphitic ones appear to be typical of a martensittic transformation of graphite into diamond known in shock processes. Such HRTEM observations give constrains on the meteorite history [5]: the diamond of this ureilite was probably formed by a shock on an already graphitised carbon. As far as disordered carbon is concerned, it could be interpreted as a post-shock thermal back-transformation of the newly synthesized nanodiamonds. 1. 2. 3. 4. 5.
Carbon molecules and Materials, éditeurs, ed. R. Setton and P. Bernier, Taylor & Francis, Londres, 2002. A. Galvez, N. Herlin-Boime, C. Reynaud, C. Clinard and J.N. Rouzaud, Carbon 40 (2002), 2775-2789 C. Le Guillou, F. Brunet, T. Irrifune, H. Ohfuji, J.N. Rouzaud, Carbon 45 (2007), 636-648. J.I. Matsuda, A. Kusumi, H. Yajima and Y. Syono, Geochim. Cosmochim. Acta, 59 (1995), 4939–4949] C. Le Guillou, J.N. Rouzaud, L. Remusat, M. Denise and A. Jambon, submitted to Geochim. Cosmochim. Acta et al
a
b
Figure 1. HRTEM images of earth analogues; a: 111 planes of diamond formed from graphite (1500°C, 15 Gpa, from [3]), and b: graphitic onion-like surrounding a nanodiamond core (heat-treatment of detonation nanodiamonds at 1100°C)
b D
a D Dis C
D
G
G
D D
Figure 2. HRTEM images of natural carbons from an ureilite meteorite (from [5]); a: nanodiamond (D) covered by disordered graphitic carbon (Dis C); b: HERTEM image and selected area electron diffraction (inset) show the parallelism of the 111 diamond planes (D) and the 002 graphite planes (G).
165
Time resolved in-situ TEM observations of Carbon Nanotube growth J. Robertson1, S. Hofmann, R. Sharma2, C. Ducati, R. Dunin-Borkowski 1. Cambridge University, Cambridge CB2 1PZ, UK 2. Arizona State University, USA [email protected] Keywords: environmental TEM, carbon nanotube, catalyst, CVD deposition, growth mechanism
Carbon nanotubes have a unique place in electron microscopy since their discovery by Iijima. They are typically produced by three methods, laser ablation, the arc and by chemical vapour deposition (CVD), usually involving a transition metal catalyst. CVD is most important because it used for industrial scale production, and also on surfaces, for making nanotubes for electronic devices [1]. However, the growth process is not well understood at an atomic level. We have studied the catalyst activation and nucleation of carbon nanotubes using in-situ time resolved transmission electron microscopy, using realistic catalysts and realistic growth conditions and pressures [2]. The catalyst activation is found to consist of a de-wetting of thin layer metal from an oxide support to form nano-crystallites. The catalyst is found to be solid and metallic under our conditions. Nucleation occurs by the formation of a carbon layer cap above the nano-particle which then grows into a nanotube. In CVD typically, one tube grows from each nano-particle. The nanotube walls grow tangentially to the catalyst surface. For multiwall nanotubes, the catalyst particle undergoes severe distortions during grown due to stress, but remains solid. Supplementary in-situ XPS studies confirm that the catalyst is in metallic rather than oxide or carbide state [3]. 1. 2. 3.
J Robertson, Materials Today 10 p36 (Jan 2007) S Hofmann et al, Nanoletts 7 602 (2007) C Mattevi, S Hofmann, et al, J Phys Chem C (accepted)
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 165–166, DOI: 10.1007/978-3-540-85226-1_83, © Springer-Verlag Berlin Heidelberg 2008
166
Figure 1. The catalyst restructures into a series of nano-particles in order to be active in growth.
Figure 2. In-situ TEM of nucleating and growing carbon nanotubes.
167
Insulator-Metal transition: formation of Diamond Nanowires in n-type Conductive UNCD films R. Arenal 1, O. Stephan2, P. Bruno3, D.M. Gruen3 1. LEM, CNRS-ONERA, 92322 Châtillon - France 2. LPS, Université Paris-Sud, 91405 Orsay - France 3. MSD, Argonne National Laboratory, IL 60439 Argonne - USA Raul.Arenal@onera fr Keywords: Nanodiamond, Nanowires, UNCD, HRTEM, EELS, Transition Insulator-Metal
Under normal process conditions UltraNanoCrystalline Diamond (UNCD) films are highly electrically insulating, but they can become highly conducting when Ar is substituted in the synthesis gas with some of N2. The potential utility of these films that provide the only currently available source of n-type diamond material conducting at ambient temperatures makes interesting to gain a better understanding of the mechanism underlying the insulator-metal transition [1]. In this communication, we present a detailed study of the microstructure of UNCD films as a function of plasma N2 content using electron diffraction, HRTEM and EELS. We performed this work in a FEI Tecnai F20 and in a VG HB501 operating at 200 and 100kV, respectively. The latter microscope provides appropriate conditions to obtain spectroscopy information at the nanometre scale on individual nanostructures [2,3]. Figure 1 (I) and (II) correspond to general views of the samples where elongated nanowires (NWs) are visible. These NWs starts to appear when the N2 content in the gas phase reaches about 10% in volume. They are ~ 100 nm in length and about 5 nm in width as shown in the TEM image (Figure 1 (II)) and more precisely in Figure 2 (I). The lattice fringes corresponding to the d-spacing of the (111) planes of diamond are visible in this latter HRTEM image [1]. The NWs are enveloped by an amorphous layer of about 1nm thick and are embedded by a matrix composed by randomly oriented 3-5 nm crystallites of UNCD. C-K edge is shown in Figure 2 for EEL spectra acquired on different positions on a sample containing those NWs. These spectra were recorded respectively on: the middle of a NW (I), the matrix (II) and the edge of a NW (III). The analysis of the fine structure of the C-K edge confirms that each NW is diamond and that they are enveloped in a sheath of sp2 bonded carbon [1,4]. Moreover we have detected the presence of nitrogen in the amorphous layer. The concentration of N is under one atomic percent. From this study we concluded that the insulator-metal transition of these films is strongly correlated with the formation of these diamond NWs. These NWs are enveloped by an amorphous carbon layer that seems to provide the conductive path for electrons.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 167–168, DOI: 10.1007/978-3-540-85226-1_84, © Springer-Verlag Berlin Heidelberg 2008
168
1. 2. 3. 4. 5.
R. Arenal, P. Bruno, D.J. Miller, M. Bleuel, J. Lal, D.M. Gruen, Phys. Rev. B (2007). R.F. Egerton, EELS in the Electron Microscope. 2nd edn. Plenum, New York (1996). R. Arenal, O. Stephan, M. Kociak, D. Taverna, A. Loiseau, C. Colliex, Phys. Rev. Lett. (05). R. Arenal, G. Montagnac, P. Bruno, D.M. Gruen, Phys. Rev. B (2007). This work was supported by the U. S. Department of Energy, Office of Science, under Contract DE-AC02-06CH11357.
Figure 1. (a) SEM and (b) low magnification TEM images of the samples showing the presence of NWs.
Figure 2. (I) HRTEM image showing one of these Diamond NWs and the matrix. (II) C-K edge for several probe positions on an n-UNCD sample corresponding with: (a) middle of a diamond NW, (b) at the edge of the NW and (c) in the matrix, respectively.
169
Field emission from iron-filled carbon nanotubes observed in-situ in the scanning electron microscope K.J. Briston1, Y. Peng1,3, N. Grobert2, A.G. Cullis3 and B.J. Inkson1 1. Department of Engineering Materials, University of Sheffield, Mappin Street, Sheffield, UK, S1 3JD 2. Department of Materials, University of Oxford, Parks Road, Oxford, UK, OX1 3PH 3. Department of Electronic and Electrical Engineering, University of Sheffield, Mappin Street, Sheffield, UK, S1 3JD [email protected] Keywords: carbon nanotubes, iron, field emission
Carbon nanotubes (CNTs) have been found to be very good field emitters with low turn-on fields and high current densities [1]. This has made them attractive as possible electron sources in, for example, cathode ray tubes and electron microscopes. Numerous studies have been conducted to date on field emission from standard, unfilled CNTs (e.g. [2-4]), which have linked the field emission properties of CNTs to their structural properties. However, there is very little data available on the field emission properties of filled CNTs, particularly individual filled CNTs. Recently work by Chai et al [5] revealed that arrays of CNTs filled with iron oxide had a lower turn-on field than both arrays of nitrogen-doped CNTs and unfilled CNTs. This raises the possibility that iron-filled CNTs could be similarly successful. In this work, individual iron-filled CNTs were mounted on an SEM nanomanipulator (Kleindiek MM3A) with a sharp electrochemically etched gold tip. A second nanomanipulator with a gold tip was moved to a distance of approximately 300nm-600nm from the freestanding end of the CNT to act as an anode during field emission (see Figure 1). Field emission was obtained from 5 separate iron-filled CNTs. The maximum current that was reached with any of the CNTs was 5.38μA. The turn-on field for the 5 CNTs ranged from 114 to 251 Vμm-1, which is comparable to the turn-on field found for unfilled CNTs using the same experimental set up. The turn-on fields measured are higher than in other works due to the reduced field concentration effect at the very small gap distances used in this work [6]. Two of the CNTs were imaged in a JEOL JEM-2010F transmission electron microscope (TEM) following field emission to view their structures and see how the iron was distributed within them. The structures observed were substantially different: one CNT (CNT-1) was relatively straight and uniform containing numerous sub-5nm iron-rich particles while the other (CNT-2) was curved and contained relatively large iron-rich particles up to ~100nm in diameter that distorted the walls of the CNT. In both cases the iron was distributed asymmetrically along the tubes, being mainly located at the bases of the CNTs. In CNT-1 a high density of iron-rich nanoparticles was located at the very tip of the nanotube (see Figure 2) which had a ~30nm carbon coating. In CNT-
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 169–170, DOI: 10.1007/978-3-540-85226-1_85, © Springer-Verlag Berlin Heidelberg 2008
170
2, cavities existed near the tip which looked to have once contained iron-rich particles. Investigations are still under way to see if other elements are present in the CNTs after field emission along with the iron. The asymmetric distribution of iron in the CNTs suggests that the iron has moved during field emission. Movement of iron inside CNTs under applied current has been observed previously and is thought to be due to thermally assisted electromigration [7]. It is possible the current passing through the CNT during field emission coupled with the very high temperature produced at the tip (up to 2000K at 1μA [8]) is enough to cause electromigration. The fact that one of the CNTs contains iron-rich nanoparticles is also interesting because no as-produced CNTs containing nanoparticles were seen. It seems that iron-rich nanowires inside the CNT (commonly observed in as-produced CNTs) were broken down into nanoparticles during field emission by the high field and temperature. 1. 2. 3. 4. 5. 6. 7. 8. 9.
Bonard J M, Kind H, Stockli T and Nilsson L A, Solid-State Electronics 45 (2001), p. 893. Kaiser M, Doytcheva M, Verheijen M and de Jonge N, Ultramicroscopy 106 (2006), p. 902. Wang M S, Peng L M, Wang J Y, Jin C H and Chen Q, Journal of Physical Chemistry B 110 (2006), p. 9397. Wang Z L, Gao R P, de Heer W A and Poncharal P, Appl. Phys. Lett. 80 (2002), p. 856. Chai Y, Yu L G, Wang M S, Zhang Q F and Wu J L, Chinese Physics Letters 22 (2005), p. 911. Saito Y, Seko K and Kinoshita J, Diamond and Related Materials 14 (2005), p. 1843. Svensson K, Olin H and Olsson E, Phys. Rev. Lett. 93 (2004), p. 145901. Purcell S T, Vincent P, Journet C and Binh V T, Phys. Rev. Lett. 88 (2002), p. 105502. The authors thank the EPSRC for a PhD studentship and funding GR/S85689/01.
Au
Au Fe-CNT
1μm Figure 1. SEM image showing a single iron-filled CNT attached to the gold tip of a nanomanipulator. The gold tip of a separate nanomanipulator is in position to act as an anode in field emission.
Figure 2. TEM image of the tip of CNT1 showing the high density of iron-rich nanoparticles located there after field emission.
171
Templated ordering of fullerenes on nanostructured oxide surfaces D.S. Deak, B.C. Russell, D.T. Newell, K. Porfyrakis, F. Silly and M.R. Castell1 1. Department of Materials, University of Oxford, Parks Road, Oxford, OX1 3PH, U.K. [email protected] Keywords: fullerenes, SrTiO3, scanning tunnelling microscopy
The packing arrangement of molecules on surfaces depends on a variety of factors including molecular shape, molecule - molecule interactions, and molecule - substrate bonding. There are numerous ways of ordering molecules on surfaces. The simplest strategy is to choose a clean surface where molecular adsorption leads to a reconstruction, but this only tends to work for small molecules. To influence larger molecules, such as fullerenes, one needs to create ordered adsorption site arrays that will act as a template. Without a template fullerenes will normally form two dimensional close-packed islands, as shown in Figure 1. My talk will cover our current work on schemes to use nanostructured oxide surfaces as templates to guide the molecular packing of fullerenes into non-close packed arrangements. By varying the surface processing conditions, and hence the stoichiometry, in the surface region of (001) and (111) oriented SrTiO3 crystals we can control which reconstructions are formed [1-5]. Extended annealing in ultra high vacuum (UHV) gives rise to the spontaneous growth of surface nanostructures [6-8]. We use Auger electron spectroscopy to show that the nanostructures are due to local phases caused by an enhanced TiOx concentration in the surface region. We have deposited a variety of empty and endohedral fullerenes (C60, C70, C82, Nd@C82, Er3N@C80) on the nanostructured SrTiO3 (001) surfaces and demonstrate that depending on the substrate conditions the molecules will order into close packed monolayers or lines [9,10]. For a particular nanostructure template we also show open grid array packing [11] as shown in Figure 2. Our latest results on SrTiO3 (111) surfaces demonstrate hexagonal ordering of C60 and C70 molecules. A particular template on this surface lines up the long axes of C70 molecules in one direction. 1. 2. 3. 4. 5. 6. 7. 8. 9.
M.R. Castell, Surf. Sci. 505 (2002), p. 1. K. Johnston, M.R. Castell, A.T. Paxton and M.W. Finnis, Phys. Rev. B 70 (2004) p. 085415. F. Silly, D.T. Newell and M.R. Castell, Surf. Sci. 600 (2006) p. L219. D.T. Newell, A. Harrison, F. Silly and M.R. Castell. Phys. Rev. B 75 (2007) p. 205429. B.C. Russell and M.R. Castell. Phys. Rev. B 75 (2007) p. 155433. M.R. Castell, Surf. Sci. 516 (2002) p. 33. D.S. Deak, F. Silly, D.T. Newell and M.R. Castell, J. Phys. Chem. B 110 (2006) p. 9246. H.L. Marsh, D.S. Deak, F. Silly, A.I. Kirkland and M.R. Castell, Nanotech. 17 (2006) p. 3543. D.S. Deak, F. Silly, K. Porfyrakis and M.R. Castell, Nanotechnology 18 (2007) p. 075301.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 171–172, DOI: 10.1007/978-3-540-85226-1_86, © Springer-Verlag Berlin Heidelberg 2008
172
10. D.S. Deak, K. Porfyrakis and M.R. Castell, Chem. Comm. (2007) p. 2941. 11. D.S. Deak, F. Silly, K. Porfyrakis and M.R. Castell, J. Am. Chem. Soc. 128 (2006) p. 13976.
Figure 1. Scanning tunnelling microscope image showing close-packed ordering of endohedral fullerenes Er3N@C80. Image width 55 nm.
Figure 2. Scanning tunnelling microscope image of molecular pairing of Er3N@C80 fullerenes on a nanstructured SrTiO3 (001) surface. Image width 31 nm.
173
Carbon nanostructures produced by chlorination of Cr3C2 and Cr(acac)3 A. Gómez-Herrero1, E. Urones-Garrote1, D. Ávila-Brande2, N.A. Katcho2,3, E. Lomba3, A.R. Landa-Cánovas4 and L.C. Otero-Díaz1,2 1. Centro de Microscopia y Citometría, Universidad Complutense de Madrid, Av. Complutense s/n, 28040 Madrid, Spain 2. Dpto. Química Inorgánica, Fac. Ciencias Químicas, Universidad Complutense de Madrid, Av. Complutense s/n, 28040 Madrid, Spain 3. Instituto de Química Física Rocasolano, CSIC, Serrano 119, 28006 Madrid, Spain 4. Instituto de Ciencia de Materiales de Madrid, CSIC, 28049 Madrid, Spain [email protected] Keywords: carbide-derived carbon, disordered carbon.
The preparation of nanocarbons and the study of their promising applications have attracted considerable attention in the last years [1,2]. Carbide-derived carbons (CDC) are a well-known group of nanostructured carbon materials, prepared by direct chlorination of the metal carbides according to the following reaction: MCx(s) + y/2 x C(s) + MCly(g). Previously, we have reported the preparation of CDC from Cl2(g) NbC [3] as well as the results of the direct chlorination of metallocenes: ferrocene [4] and cobaltocene [5]. In this work we are presenting the characterization of nanostructured carbon samples obtained from Cr3C2 and from Cr(acac)3 - acac: acetylacetonate, (C5H7O2)- -, mainly by means of TEM and associated techniques (EDX, EELS), employing a CM 200FEG microscope. The sample prepared from Cr3C2 at 400 ºC (reaction time: 60 minutes) consists of remains of the starting precursor encapsulated in a newly generated disordered carbon coating (see Figure 1a). When the reaction temperature is 900 ºC, SEM micrographs indicate that this CDC sample consists of faceted particles with micrometric size (see Figure 1b). TEM images show that most of them are formed by highly ordered graphitic carbon. Remains of the generated CrCl3 are observed as mono-layers between the graphene sheets, as it is shown in Figure 2a, where CrCl3 is imaged along the [010] direction. Besides, carbon particles with disordered structure are also found in this sample in lower proportion. The sample prepared by direct chlorination of Cr(acac)3 at 900 ºC (reaction time of 30 minutes) consists of irregular particles with porous surface according to SEM micrographs. TEM studies indicate that they present a highly disordered structure, with local stacking of ∼3-5 graphene layers (4-5 nm long), as it is shown in Figure 2b. EDX analyses indicate the presence of traces of Cr and Cl. EELS experiments reveal that the carbon bonding in the highly-ordered CDC particles obtained from Cr2C3 at 900 ºC is ∼ 93% sp2-type, a very close value to the ∼90% proportion found in the sample prepared from Cr(acac)3.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 173–174, DOI: 10.1007/978-3-540-85226-1_87, © Springer-Verlag Berlin Heidelberg 2008
174
1. 2. 3.
M. Inagaki, K. Kaneko and T. Nishizawa, Carbon 42 (2004), p. 1401. Y. Gogotsi, “Nanomaterials Handbook”, (CRC Press, Boca Raton) (2006). D. Ávila-Brande, N.A. Katcho, E. Urones-Garrote, A. Gómez-Herrero, A.R. Landa-Cánovas and L.C: Otero-Díaz, Carbon 44 (2006), p. 753. E. Urones-Garrote, D. Ávila-Brande, N.A. Katcho, A. Gómez-Herrero, A.R. Landa-Cánovas and L.C. Otero-Díaz, Carbon 43 (2005), p. 978. E. Urones-Garrote, D. Ávila-Brande, N.A. Katcho, A. Gómez-Herrero, A.R. Landa-Cánovas, E. Lomba and L.C. Otero Díaz, Carbon 45 (2007), p. 1699. We kindly acknowledge the financial support from the project MAT2007-63497
4. 5. 6.
b
a
500 nm
Cr3C2
5μm
Figure 1. a) TEM image of a typical particle of the sample prepared from Cr3C2 at 400 ºC; b) SEM micrograph of the CDC sample obtained at 900 ºC.
a
b hk reflections of a graphene layer
Graphite like hkl reflections
CrCl3
Figure 2. a) HRTEM image showing rests of CrCl3 (arrowed) in a CDC particle prepared from Cr3C2 at 900 ºC; b) HRTEM image of a carbon particle obtained from Cr(acac)3 (900 ºC), showing disordered structure with local stacking of graphene layers (arrowed). The corresponding electron diffraction patterns of the whole particle are inset
175
Structural peculiarities of carbon onions, formed by different methods B.A. Kulnitskiy, I.A. Perezhogin, V.D. Blank 1. Technological Institute for Superhard and Novel Carbon Materials (TISNCM), Centralnaya Street 7a, 142190 Troitsk, Moscow region, Russia [email protected] ru Keywords: onion, high pressure, TEM
Carbon onions are concentric multishell fullerene clusters of a few nanometers in size. They can be generated by various techniques. The purpose of the present study is to investigate structural peculiarities of carbon onions, formed under different conditions. The onions in our study were formed by four methods: arc-discharge between two graphite electrodes, high pressure and shear deformation treatment of graphite in the diamond anvil high pressure cell, shock-wave loading of graphite and thermobaric treatment of C60. We examined the onions by using the JEM-2010 highresolution transmission electron microscope, equipped with an EDS detector and the JSM 5800 scanning electron microscope [1, 2]. Following characteristics of carbon onions were examined: shape and amounts of shells, spacing between shells, inner structure and defects. It was shown that mainly high-quality spherical carbon onions, consisting of not more then 10 layers, were produced by the shock-wave loading. Onions, formed by other methods, range from 4 nm to 0.5 µm (5-80 spherical layers). Concentration of defects increased from low value for onions of little size to very high value for onions of big size. The presence of defects is typical for multi-layer onions produced both by high pressure treatment and by arc-discharge. Defects of different types were observed. The amount of concentric shells in onions, formed in diamond anvil high pressure cells, tended to increase with pressure and deformation growth. Large carbon onions, formed under these conditions, consist of more then 60 spherical shells. Applied external pressure resulted in formation of defects in radial direction in onions of big size. Defects represented radial lines, corresponding to the rupture of spherical packing and their displacements by the distance of half interlayer spacing. Ruptured spheres connection can be realized by the formation of sp3-bonds [3]. The spacing between outer shells of the onion as well as the spacing between inner shells is larger than the spacing between intermediate shells. Splitting of some layers in multi-layer carbon onions, produced by arc-discharge, can be explained probably by the non-equilibrium growth process. Very high concentration of defects was found in multi-layer onion-like carbon, formed under thermobaric treatment of C60 (15 GPa, 1100K). 1.
V. D. Blank, V. N. Denisov and A. N. Kirichenko, Nanotechnology, 18 (2007), p. 345601.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 175–176, DOI: 10.1007/978-3-540-85226-1_88, © Springer-Verlag Berlin Heidelberg 2008
176
2. 3.
V. D. Blank, A. A. Deribas, and B. A. Kulnitskiy, Materials science Forum 566 (2008), p. 357. A. T. Balaban, D. J. Klein and C. A. Folden, Chem. Phys. Lett 217 (1994), p. 266.
Figure 1. a) Carbon onion, formed by arc discharge, consists of about 80 spherical shells; b) Defects in the spherical packing. c) The diagram, explaining sp3-bonds generation in the case of a “failure” in shell’s periodic arrangement.
Figure 2. a) Carbon onion, formed in graphite at 71 GPa and 5 cycles of shear deformation, consists of 60 spherical shells; b) Radial lines in the onion, shown by arrows, correspond to the rupture of spherical packing and their displacements by the distance of half interlayer spacing. Ruptured spheres connection can be be realized by the formation of sp3-bonds.
177
Electron Energy Loss Spectroscopy of La@C82 peapods R.J. Nicholls1, D.A. Eustace2, D. McComb2, G.A.D. Briggs1, D.J.H. Cockayne1 and D.G. Pettifor1 1. Department of Materials, University of Oxford, Parks Road, Oxford OX1 3PH, UK 2. Department of Materials, Imperial College London, London SW7 2AZ, UK rebecca [email protected] Keywords: EELS, carbon nanomaterials, La@C82
Carbon nanomaterials, such as fullerenes and nanotubes, have potential applications, such as drug carriers [1] and in quantum nanotechnology [2]. In order to use these materials fully, it is necessary to have a good understanding of their properties and how to alter them. Electron energy loss (EEL) spectroscopy provides a probe of the unoccupied density of states (DOS) of a material. Monochromation of the electron source means that it is possible to get high electron energy resolution, which, along with simulated spectra, can be used to obtain a better understanding of the electronic structure of a material. Previously this combination of experiment and theory has been used to look at fullerene crystals [3], and to determine the effect of changes in bond length on the DOS and EEL spectra [4]. We are now extending this investigation to look at the interaction between a carbon nanotube and fullerenes encapsulated inside it. We are using the newly installed monochromated FEI TITAN at Imperial College London to acquire high energy resolution spectra from La@C82 nanocrystals and single-walled nanotubes filled with La@82. This microscope can be operated at 100 kV with energy resolution ~0.15 eV. Monochromation is essential to this study as we are looking for small differences in the fine structure of the edge. A schematic diagram of La@C82 molecules encapsulated inside a single-walled nanotube is shown in Figure 1. The major isomer of La@C82, which is thought to have C2v symmetry, has been used to make the nanocrystals and to fill the nanotubes. The carbon K-edge from La@C82 is shown in Figure 2a, alongside that from C82. Pristine C82 is thought to have C2 symmetry. The π* peak in the C82 appears narrower than that in the La@C82, which is not surprising as there is less symmetry in the La@C82 case. Figure 2b shows examples of two carbon K-edges from the La@C82 peapod sample. Figure 2b(i) is a spectrum from an area of the sample containing lanthanum and Figure 2b(ii) is from an area which does not contain lanthanum. The area which does not contain lanthanum is likely to be an unfilled nanotube. This is supported by the similarity of the spectrum to that of a single walled nanotube. Apart from the relative heights of the π* and σ* peaks, there are two main differences between the spectra which are a shift in the peak labelled A, and a decrease in the peak labelled B in the case without lanthanum. Our combination of experiment and modelling is the only way to understand the origin of these differences.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 177–178, DOI: 10.1007/978-3-540-85226-1_89, © Springer-Verlag Berlin Heidelberg 2008
178
1. 2. 3. 4.
A. Hirsch, Physica Status Solidi B 243 (2006), 3209. J.J. Morton et al., Nature Physics 2 (2006), 40. S.M. Lee et al., Chemical Physics Letters 404 (2005), 206. R.J. Nicholls et al., Micron 37 (2006), 449.
(a)
(b)
Figure 1. Schematic drawing of (a) a La@C82 molecule and (b) a single-walled nanotube filled with La@C82 molecules.
a Intensity (arb. scale)
i ii
-2
0
2
4
6
8
10
12
14
16
18
20
Energy loss above edge onset (eV)
1.2
b
A
Intensity (arb. scale)
1
B
0.8
with La (i) without La (ii)
0.6 0.4 0.2 0 -5
5
15
25
35
Energy loss above edge onset (eV)
Figure 2. Carbon K-edges from: (a) (i) La@C82, (ii) C82; and (b) a sample of nanotubes containing La@C82, including (i) an area containing La and (ii) an area without La.
179
HRTEM studies of Y-junction bamboo-like CN-nanotubes I.A. Perezhogin, B.A. Kulnitskiy, V.D. Blank, D.V. Batov, E.V. Polyakov 1. Technological Institute of Superhard and Novel Carbon Materials, Centralnaya str. 7a, Troitsk, Moscow region, 142190 Russia [email protected] Keywords: Y-junction, carbon nanotube, transmission electron microscopy
Carbon branched structures are of interest because of their novel functionality and possible applications. Seamless junctions between carbon nanotubes (CNT) are obtained due to the topological defects (i. e. pentagons, heptagons, octagons, etc.) in the hexagonal lattice. In order to obtain multiwall Y-junction bamboo-like CNx nanotubes we use a technique of resistive heating of graphite in a water-cooled hot isostatic pressure apparatus (HIP). Argon-nitrogen mixture (with molar ratio 1:2.5) was used as a gas medium. We did not place any catalyst material into the reaction volume on purpose, but we used a mullite wool as one of the heat screen parts, and we believe, that the mullite wool was a source of Mg, Si, Ca, and Al found in catalyst particles of nanotubes. CNx nanotubes were characterized by transmission electron microscope JEM-2010 equipped with the EDS (Energy Dispersive X-Ray Spectroscopy) system. The TEM images have shown that the material consists of many Y-junctions with the main CNT stem and CNT branches. In most cases the angles between the branches are close to 120°. The nanotubes are 80—170 nm in diameter and have either one or several Y-junctions. Y-junction nanotubes both with short and long branches were observed. It is interesting that the short branches as well as those grown at the end of the process have a conic shape. Usually nanotubes are divided into identical compartments, but some of the observed nanotubes have the compartments of larger length. It is seen that all the Y-junction bamboo-like CNx nanotubes contain pear-shaped catalytic particles at the end. It is believed that the growth of branching structures occurs mainly due to the change of both physical and chemical properties of catalyst particles caused by different reasons. Undoubtedly, catalyst nanoparticles are liquid at temperatures above 1400 °C and thus can take any shape during the nanotubes growing process. Inhomogeneous concentration of carbon in the bulk of the catalyst particle and on its surface may result in drastic change of growth conditions at different parts of the catalyst, thus resulting in the growth of branching structures (when the growth stops in certain area and begins at the other place of the catalyst). Figure 1 shows that the temperature change due to, for example, the fluctuation of gas flow in the reactor results in the change of the carbon solution and location of precipitation sites. New deposition site is bordered by black arrows. The nanotube branch growth proceeds in the other direction. The growth in the former direction (figure 1) stops because the direction of the diffusion of the carbon atoms has been changed. It is worth to notice, that the growth of the “stem” of nanotube proceeds by the tip-growth mechanism, which means that a nanotube growth direction is opposite to the direction of carbon diffusion to the precipitation site, and the growth of the “branches” follows the base-growth mechanism which implies the coincidence of S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 179–180, DOI: 10.1007/978-3-540-85226-1_90, © Springer-Verlag Berlin Heidelberg 2008
180
the abovementioned directions inside a particle. We believe that CN radicals play a decisive role in growing the bamboo-like nanotubes as they take part in the formation of pentagons needed for the precipitation of curved graphene layers on a catalyst particle surface.
Figure 1. Y-junctions formed in the HIP apparatus.
181
EF-TEM observation of biological tissue for risk assessment of fullerene nanoparticles K. Yamamoto1, M. Makino1, E. Kobayashi1 and Y. Morimoto2 1. National Institute of Advanced Industrial Science and Technology (AIST), Higashi, Tsukuba, Japan 2. University of Occupational and Environmental Health, Iseigaoka, Kitakyushu, Japan [email protected] Keywords: fullerene, risk assessment, EF-TEM
Industrial applications of nano-carbon materials such as fullerenes, carbon nanotubes, and nanocrystalline diamonds were reported in many fields recently. The toxicity of these nano-carbon materials for the human was not clear, therefore, the toxicity test and risk assessment were very important. Transmission electron microscope (TEM) was powerful technique to study the nano-world, and used both material and biological research. In the case of the observation for the biological cells, the high contrast observation was important, and then, the cell specimens were usually stained with the heavy elements such as U and Pb to increase the contrast of image. However, it was difficult to observe the stained specimen of biological cells containing carbon nanosized carbon materials, because the contrast from carbon nano-sized particles was weak and below the background of the staining heavy elements. Furthermore, the highresolution observation is necessary for the nanoparticles in the biological cells. In this study, the zero loss imaging of the biological tissue with fullerene nano-sized particles is examined by using an energy-filtering TEM with the objective lens for the high-resolution imaging (Zeiss, EM922HR). The acceleration voltage was 200 kV. The electron spectroscopic zero-loss images, which are filtered at a loss energy of 0 eV with an energy window-width of 20 eV, are formed with both unscattered and elastically scattered electrons. The scattering contrasts, Bragg contrasts, and phase contrasts in the filtered zero-loss images are higher than those in the unfiltered images. The in-vivo test of fullerenes was the intratracheal instillation of fullerenes solution in the rat lung. The test solution was the fullerene nanoparticles in the water with 0.1g/l Tween 80 dispersions. The TEM images of fullerenes in the test solution are shown in Figure 1(a) and (b). The diameter of fullerenes is 20 nm, and the fullerene is crystalline. The mount of fullerenes in the solutions were 100 or 200 μg. The fullerene solution was intratracheally instilled in rat lung. The lung tissues after one week, one month, and three months from the instillation were observed by TEM. The lung tissue was fixed using glutaraldehyde and osmium tetroxide solution, and then dehydrated in ethanol, and embedded in epoxy resin. Ultrathin sections were cut on a diamond knife with microtomy. The staining condition of the tissue specimen was examined. The TEM zero loss image of the alveolar macrophages after one week instillation exposure was shown in Figure 2 (a), and the high resolution image of the black particles indexed by an arrow in Figure 2 (a) was shown in Figure 2 (b). According to the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 181–182, DOI: 10.1007/978-3-540-85226-1_91, © Springer-Verlag Berlin Heidelberg 2008
182
electron diffraction analysis of these particles, these are identified as the fullerenes. Fullerenes particles keep the fcc crystal structure. As the diameter of fullerenes in Figure 2 (b) was 20 nm, fullerenes keep the particle size. The most of fullerenes particles are observed in the alveolar macrophages and a part of fullerenes are in the alveolar cells. Fullerenes still remained in the alveolar macrophages and the alveolar cells after one month or 3 months instillation exposure.
Figure 1. Low magnification image of the fullerene particles in the test solutions (a). The diameter of the fullerene particle is 20 nm, and the lattice of (111) is observed (b).
Figure 2. Low magnification image of the alveolar macrophages in the rat lung after one week from the instillation (a). (b) is the high-resolution image of the particles indexed by a white arrow in (a). This work was supported by New Energy and Industrial Technology Development Organization (NEDO) of Japan.
183
Looking at the surface of catalysts nanopowders J.C. Hernandez, A.B. Hungria, M. Lopez-Haro, J.A. Perez-Omil, S. Trasobares, S. Bernal, P. Midgley, O. Stephan, J.J. Calvino 1. Dept. de Ciencia de los Materiales e Ingeniería Metalúrgica y Química Inorgánica, Universidad de Cadiz, Campus Rio San Pedro s/n, Puerto Real 11510 (Cadiz), Spain 2. Department of Materials Science and Metallurgy. University of Cambridge, Cambridge, CB2 3QZ, UK 3. Laboratoire de Physique des Solides, Universite Paris Sud, 91495 Orsay, France [email protected] Keywords: Catalysts, surface structure, surface composition
Although the bulk it is usually also involved in supporting catalytic processes, it is clear that surface is the key site of these phenomena. Understanding the complex catalytic action requires detailed information about how synthesis, activation or function itself change structural and compositional features of the surface. Most of the techniques currently available at modern electron microscopes are not surface specific but they provide rich information about this particular location. In this contribution we discuss different cases which illustrate some of the potential capabilities of TEM-STEM in the analysis of the structure and composition of the surface of powdered complex multicomponent catalytic materials based on lanthanide oxides. Thus, the complementary use of STEM-HAADF tomography and atomic imaging by HREM and HAADF has proved essential to understand the changes in the redox behaviour of CexZr1-xO2 mixed oxides [1,2]. These materials, used in the formulation of the catalytic converters of the exhaust gases of gasoline-powered cars, improve their oxygen handling capabilities after specific aging treatments in reducing atmospheres at high temperatures. HREM imaging points to the formation in the bulk of a superstructure as responsible of the improvements of the redox properties. On its hand, HAADF has revealed that this superstructure is related to a disorder-order transition in the cationic sublattice of the oxides. Such structural transition nucleates on the surface and evolves throughout the rest of the bulk giving rise, as revealed by 3D-tomographic reconstruction, to oxide nanocrystallites dominated by {111}-type exposed surfaces. Such surfaces have been proved, by STEM-HAADF images, to be Zr-rich variants of an oxidised pyrochlore-type superstructure of the CexZr1-xO2 oxides. Figure 1. The formation/destruction of these Zr-rich, cation-ordered, {111}-surfaces correlates with the changes in the surface chemistry properties of these oxides [3]. The whole set of data to be presented will demonstrate how a combined use of different (S)TEM techniques provide the necessary information to rationalize a really puzzling chemical problem as it is that of the redox behaviour of the Ce-Zr mixed oxide family. A second example will highlight the contribution of nanoanalysis by STEM-XEDS and STEM-EELS. Results obtained in an in-depth characterization of a series of catalysts based on CexPr1-xO2-δ mixed oxides will be presented. These oxides have been studied as redox components of both Metal/CexPr1-xO2-δ and, more complex, Metal/ CexPr1-xO2-δ /doped-Al2O3 catalysts. Nanoanalytical evidences have been crucial to S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 183–184, DOI: 10.1007/978-3-540-85226-1_92, © Springer-Verlag Berlin Heidelberg 2008
184
understand the different chemical processes involved in the synthesis of these metalloaded materials and which strongly affect the surface features of both the original oxides and the metal nanoparticles [4]. Likewise, nanoanalytical tools provide clues about the role of alumina dopants to prevent redox activity decay, due to high temperature aging, in the case of the multicomponent Metal/ CexPr1-xO2-δ /doped-Al2O3 materials. In summary, the results to be presented provide a clear picture of how the appropriate use of a combination of Electron Microscopy techniques becomes a unique tool to reveal the subtle, highly localised, surface modification processes which control the macroscopic performance of powder, nanocrystalline, catalysts. 1. 2. 3. 4. 5.
J.A. Perez-Omil, S. Bernal, J.J Calvino, J.C. Hernandez, C. Mira, M.P. Rodríguez-Luque, R. Erni, N.D. Browning, Chem. Mater., 17(17) (2005), 4282. J.C. Hernandez, A.B. Hungria, J.A. Perez-Omil, S. Trasobares, S. Bernal, P.A Midgley, A. Alavi, J.J. Calvino, J. Phys. Chem. C, 111 (26) (2007), 9001. M.P. Yeste, J.C. Hernandez, S. Bernal, G. Blanco, J.J. Calvino, J.A. Perez-Omil, J.M. Pintado, Chem. Mater., 18(11) (2006), 2750. M.P. Rodriguez-Luque, J.C. Hernandez, M.P. Yeste, S. Bernal, M.A. Cauqui, J.M. Pintado, J.A. Perez-Omil, O. Stephan, J.J. Calvino and S. Trasobares, J. Phys. Chem. C (2007) (in press)† We acknowledge the financial support from Ministry of Education and Science of Spain (MAT2005-00333) and Junta de Andalucia (FQM334, FQM110). Part of the Electron microscopy work was carried out at the Electron Microscopy Division of the Central Services of Science and Technology at the University of Cádiz. The authors acknowledge financial support from the European Union under the Framework 6 program under a contract for an Integrated Infrastructure Initiative. Reference 026019 “ESTEEM”.
Figure 1. (left) 3D reconstruction of a Ce0 68Zr0 32O2 nanocrystallite showing octahedral shapes; (right) HAADF image showing alternation of Ce and Zr rich (111) planes in the Ce0 68Zr0 32O2 oxide with pyrochlore type superstructure. The first plane at the surface corresponds to a Zr-rich variant (lower image intensity in the intensity profile below).
185
Gathering structural and analytical information on catalysts at sub-nanometer level with TEM F.J. Cadete Santos Aires and M. Aouine IRCELYON, Institut de Recherches sur la Catalyse et l’Environnement de Lyon. UMR 5256 CNRS/Université Lyon 1. 2, Avenue Albert Einstein. 69626 – Villeurbanne cedex. France [email protected] Keywords: catalysts, TEM
Catalytic reactions are based on the adsorption and possible dissociation of reactants at the surface of catalysts. The prevailing role of the catalyst surface implies the use of very divided materials in order to increase the surface/bulk atom ratio leading to better efficiency and specific properties of the catalysts as well as to atom economy. Catalysts are thus generally formed by nanoparticles (metals, oxides, sulphides, …) supported on low-density materials (which are also more or less divided according to the final application). Most of the characterization techniques used to study these materials are not spatially-resolved and can only give global information on the properties of the catalysts. Since catalysts are composed of nanomaterials it is essential to be able to gather information at sub-nanometer level. Transmission electron microscopy, together with associated analytical techniques, is able to probe the properties of materials at subnanometer and atomic levels and gather localized information on morphology, composition and atomic-structure variations within the catalyst. Such information leads to a good knowledge of the catalyst and is essential to understand its catalytic behavior in relation with its local physico-chemical properties. It is thus in many cases a key and unique technique to elucidate the catalytic behavior of the catalysts (specific activity and selectivity, poisoning and deactivation, …) as well as to give directions for the synthesis of new catalytic materials with specific properties (activity, selectivity, multifunction, resistance to poisoning…). Examples illustrating these aspects [1-5] will be given in this presentation. 1. 2. 3. 4. 5.
F.J. Cadete Santos Aires et al., Proc. EUREM XII (Brno), Vol.II (Physical Sciences), 2000, 395-396. M. Aouine et al. (unpublished). M. Aouine et al., Chem. Commun., 2001, 1180-1181. F.J. Cadete Santos Aires et al., Catal. Today 117 (2006) 518-524. R . Mahfouz et al., Applied Surface Science 254 (2008) 5181-5190.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 185–186, DOI: 10.1007/978-3-540-85226-1_93, © Springer-Verlag Berlin Heidelberg 2008
186
b
0.225 nm
0 20 nm
0.195 nm
0.23 nm
Pd
0.23 nm
0.225 nm
counts 0.267 nm
PdO
Au
Pd
Pd81Au19
0.265 nm
c
α-Si3N4 (2 0 1) 0.288 nm
Energy ( keV)
Figure 1. (a) co-existence of Pd and PdO nanoparticles supported on α-Si3N4 in a fresh catalyst for the combustion of methane ; (b) PdAu nanoparticle synthesized by laser ablation in vacuum and the corresponding EDX spectrum (d).
b
a
Figure 2. Deactivation of a catalyst : PdO nanoparticles on β-Si3N4 totally (a) and partially (b) coated during methane combustion.
a
a
b
b
c
Figure 3. Identification of a new active phase in the selective oxidation of propane towards acrylic acid (MoV0 33Te0 22Nb0 11Ox) : (a) experimental image; (b) model ; (c) simulated image.
187
Size effect and influence of nanoparticles thickness on order/disorder phenomena in CoPt nanoparticles D. Alloyeau1,2, C. Ricolleau1, T. Oikawa1,3, C. Langlois1, Y. Le Bouar2 and A. Loiseau2 1.
MPQ, Univ. Paris 7 / CNRS, UMR 7162, Bâtiment Condorcet, 75205 Paris, France 2. LEM, ONERA / CNRS, UMR 104, B.P. 72, 92322 Châtillon, France 3. JEOL (Europe) SAS, 1 Allée de Giverny, 78209 Croissy-sur-Seine, France
[email protected] Keywords: CoPt nanoparticles, Order/disorder phenomena, Electron tomography
The present work is focused on the study of the size effect on the thermodynamical behaviour of CoPt nanoparticules. Equiatomic CoPt bulk present a phase transition at 825°C, between a tetragonal ordered phase (L10) at low temperature and a disordered Face Centered Cubic (FCC) structure at high temperature. Order-disorder phenomena and the order state of CoPt nanoparticles are investigated as a function of the size and shape of the nanoparticles using Transmission Electron Microscopy (TEM). The synthesis of CoPt nanoparticles is performed by alternative deposition of Co and Pt atoms by using the pulsed laser deposition technique (PLD) with a KrF excimer laser (λ=248 nm) in a high vacuum chamber. Nanoparticles are elaborated on thin amorphous carbon films. By means of an in situ heating experiment in a TEM [1] we have determined that the ordering and the growth of the particles occur when the temperature is over 600°C and 700 °C respectively. To observe the size effects on the order-disorder phenomena, disordered particles samples with a mean particle size of 2 and 3 nm have been annealed during 1 hour at 650°C, 700°C and 750°C. The nanoparticles structure as a function of their size has been determined using the STEM / NBD technique that we have recently developed [2]. Consistently with previous works [3], we did not find ordered particles smaller than 3 nm (Figure 1) in the sample annealed at 650°C. This result evidences a decreasing of the order / disorder phase transition temperature from 825°C to at least 650°C for nanoparticles size smaller than 3 nm. Moreover, particles with the same size in the substrate plane are found with different structural state i.e. L10 or FCC (Figure 2). The 3D morphology of the nanoparticles has been also studied by electron tomography experiments (Figure 3). The particles exhibit ellipsoidal shapes and depending on their size and the annealing temperature, the nanoparticles are more or less elongated in the plane of the substrate. Using both electron tomography and HRTEM focal series we determined that disordered nanoparticles have smaller thickness (≤ 2nm) than the ordered nanoparticles (≥ 3 nm). These results show that order-disorder phenomena in CoPt nanoparticles are strongly dependent not only on the nanoparticles size but also on their 3D morphology. 1. 2. 3.
D. Alloyeau et al., Nanotechnology 18 (2007) p. 375301. D. Alloyeau et al., Accepted in Ultramicroscopy (2008). T. Miyazaki et al. Physical Review B 72 (2005), p. 144419.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 187–188, DOI: 10.1007/978-3-540-85226-1_94, © Springer-Verlag Berlin Heidelberg 2008
188
Figure 1. STEM BF image of CoPt nanoparticles annealed at 700°C (left). Nano Beam Diffraction pattern of nanoparticles (b) and (c) shown in the BF image (right).
Figure 2. HRTEM images of CoPt nanoparticles annealed over 650°C : (a) disordered particles oriented along the <100> zone axis. Ordered particles oriented along the (b) [001] and (c) [110] zone axes.
Figure 3. (a) Tomogram of CoPt nanoparticles annealed at 750°C. (b) Enlargement of the tomogram showing the slicing of the tomogram in the (x,z) plane (horizontal white line) and the (y,z) plane (vertical white line) allowing the measurement of the nanoparticle thickness.
189
In situ L10 ordering of FePt nanoparticles P. Bayle-Guillemaud1, M. Delalande2, V. Monnier3, Y. Samson2 and P. Reiss3 CEA-Grenoble, Institut Nanosciences et Cryogénie, 17, Rue des Martyrs 38054 Grenoble cedex 9, France 1. SP2M/Laboratoire d’Etudes des Matériaux par Microscopie Avancée 2. SP2M/Nanostructures et Magnétisme 3. SPrAM/LEMOH pascale.bayle-guillemaud@cea fr Keywords: FePt nanoparticles, L10 ordering, TEM
Assemblies of monodisperse FePt nanoparticles (NPs) are promising candidates for next generation data storage media with recording densities beyond 1 Tbit.inch due to their high uniaxial magnetocrystalline anisotropy, which can reach 107 J m-3 along the [001] direction of the face-centered tetragonal (fct) L10 ordered phase.2 Triggered by the seminal work of Sun and coworkers [1] the chemical synthesis of FePt NPs has been extensively studied for the last few years. As-synthesized NPs exhibit a chemically disordered fcc structure. Therefore a post-synthetic treatment of the NPs, such as thermal annealing, is necessary to transform the fcc structure into the ordered fct structure which exhibits the magnetic anitotropy . This phase transition is only possible for close to equimolar stoichiometry (Fe50Pt50) NPs. In this work we present results of in situ annealing of two populations of NPs. The NPs are chemically synthesised, more details can be found in [2]. Two samples of NPs (I and II) are investigated in this work with different synthesised parameters. The first sample (I) exhibits NPs of 7nm with a core/shell structure as shown on the EFTEM analysis of Figure 1. The core being Pt rich and the shell being a 1 nm Iron oxide component. The sample II is made of bimodal size distribution: both spherical NPs with about 4 and 14 nm diameter respectively are observed. The TEM experiments were done on a 3010 JEOL microscope equipped with a Gatan Image Filter (GIF). In situ annealing was made using a JEOL specimen holder allowing heating up to 800°C. HREM images have been taken during experiment. STEM/HAADF images have been obtained afterwards on a FEI-Titan microscope equipped with a Cs-probe corrector. For both sample, in situ annealing above 500°C reveals L1O ordering of the NPs. The ordering is firstly detected at the shell of the NPs. For sample I, this could be explained by the diffusion of the Fe species to the core of the NPs before to reach a composition close to Fe50Pt50. Figure 2a shows an HREM pictures with lighter planes (001) with a double fringe spacing with respect to the 002 lattice distance which is due to the L10 ordering. The same process is observed for the two populations of sample I (Figure 2b). These latter NPs have also been observed by Z-contrast (Figure 2c). This Zcontrast imaging reveals more easily the fraction of small and large particles ordered
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 189–190, DOI: 10.1007/978-3-540-85226-1_95, © Springer-Verlag Berlin Heidelberg 2008
190
after the annealing process. A 600°C annealing temperature is necessary to get full ordered NPs. 1. 2.
Sun, S; Murray, C. B.; Weller, D.; Folks, L.; Moser, A. Science. 2000, 287, 1989-1992 V. Monnier, M. Delalande P. Bayle-Guillemaud, Y Samson and P. Reiss, Small (to be published 2008)
Figure 1. EFTEM images and chemical profile across particles obtained before annealing on Fe(L23), O(K) and Pt(M45) edge of the NPs of sample I showing the coreshell structure and sample II showing homogeneous Fe and Pt distribution.
Figure 2. a and b ) in situ HREM image of the L10 ordering of sample I (a) and II (b). The 001 planes showing the L10 ordering are observed in both case after annealing above 500°C. c) shows a STEM/HAADF image showing alternative bright and darker planes due to Z contrast of the Fe and Pt alternative planes of the L10 chemical ordered structure .
191
Characterization of indium doped zinc oxide nanorods H. Burghardt1, H. Schmid1, W. Mader1 1. Rheinische Friedrich-Wilhelms-Universität, Institut für Anorganische Chemie, Römerstr. 164, 53117 Bonn, Germany [email protected] keywords: diffraction contrast, EDX, In-doped zinc oxide nanorod,
Nanorods are a specific group of quasi one-dimensional materials. A wide range of chemical compounds have been synthesized by various growth techniques over the past decade. Zinc oxide (ZnO) is an n-type semiconductor with a band gap of 3.44 eV at 4K and shows interesting electrical and optical properties. The properties of ZnO can be widely varied by doping with different metal oxides. In this contribution ZnO nanorods are doped with indium oxide. The nanorods were grown via the vapour-liquid-solid (VLS) process [1], which is a metal catalyst supported vapour deposition mechanism. Au catalyst particles deposited on fused silica was used as substrate. A mixture of ZnO, In2O3 and graphite powder was used as sources for zinc, indium and oxygen vapour, respectively. The experiments were performed in a furnace with two heating zones and with argon as carrier gas. The substrate temperature was held at 950°C. The nanorods grow in the direction of the ZnO c-axis despite a short kinked segment at the end of the rod. (fig. 1). The nanorods are crystalline and exhibit a characteristic domain structure (fig. 2) with inversion domain boundaries (IDBs) known from bulk In2O3(ZnO)m material [2, 3]. There exist two types of IDBs, parallel to basal planes and parallel to prism planes of ZnO, respectively, which appear in a strictly alternating sequence. The boundaries are best distinguished in dark field images by an abrupt change of diffraction contrast (see fig. 2b). It is known from studies on bulk materials that the spacing of basal plane IDBs determines the local In content in these systems [3]. The density of IDBs in the rod shown in fig. 2 yields an In content of 0.3 at.% (with respect to Zn) under the assumption of one monolayer of In per IDB. Careful chemical analysis of the nanorod segment using EDX in STEM yielded 0.6 at.% In which is twice the In content which would be measured in bulk In2O3(ZnO)m material. The study of this discrepancy is the subject of ongoing research. 1. 2. 3.
R. S. Wagner, W.C. Ellis, Appl. Phys. Lett. 4 (1964), 89-90. A. Loewe, Ph.D. thesis, University of Bonn (2001). C.Li.Y. Bando, M. Nakamura, N. Kimizika, J. Electron Microsc 46 (1997), 119-127
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 191–192, DOI: 10.1007/978-3-540-85226-1_96, © Springer-Verlag Berlin Heidelberg 2008
192
Figure 1. In-doped ZnO nanorod grown along (0001) on holey carbon film with gold catalyst particle at the end.
Figure 2. In-doped ZnO nanorod with inversion domain microstructure and IDBs marked by arrows. Bright field (a) and corresponding (0002) dark field image.
193
Adsorbate-induced restructuring on Pt nanoparticles studied by environmental transmission electron microscopy M. Cabié, S. Giorgio and C.R. Henry CINAM-CNRS, Campus de Luminy, Case 913, 13288 Marseille cedex 9, France [email protected] Keywords: Environmental TEM, Pt catalysts, surface restructuring
The reactivity of metal nanoparticles depends on their shape, their structure and their morphology. Furthermore, the adsorption of reactive species on the surface of these catalysts can modify their morphology. These considerations illustrate the need of in situ characterization in order to better understand the elemental mechanisms of catalytic reactions. The in situ imaging of Pt catalysts deposited on amorphous carbon has been performed under gas pressure with environmental transmission electron microscopy (ETEM). The E-TEM microscope is a standard TEM equipped with an environmental sample holder allowing the insulating of the sample towards the vacuum of the TEM column [1]. Perfectly homogeneous Pt catalysts exhibiting well-defined shape have been chosen to follow surface restructuring induced by gas exposure. These nanoparticles obtained by the decomposition of organometallic compounds present different morphologies with a majority of particles with square outlines as illustrated in Figure 1. According to HRTEM and weak beam dark field (WBDF) imaging, most of the particles are cubes truncated with more or less extended {111} and eventually {110} facets. These particles size is in the range between 10 and 30 nm. Morphological changes have been observed on a same cluster during gas treatments similar to those usually applied to supported metal catalysts, i.e. oxidation-reduction treatments under a pressure of 5 mbar. Under hydrogen, a faceting of the particle is clearly evidenced (see Figure 2). After oxidation of this same particle a continuous rounding of the particle profile is observed: the corners become rounded and the edges roughen. This rounding of the particle profile indicates higher index facets are formed (see Figure 2). Results in agreement with this study were reported for supported Pt catalysts observed ex situ by TEM [2, 3]. 1. 2. 3.
S. Giorgio, S. Sao Joao, S. Nitsche, D. Chaudanson, G. Sitja and C. R. Henry, Ultramicroscopy 106 (2006), p. 503. G. Rupprechter and H. J. Freund, Topics in catalysis 14 (2001), p. 1. A. S. Ramachandran, S. L. Anderson and A. K. Datye, Ultramicroscopy 51 (1993), p. 282.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 193–194, DOI: 10.1007/978-3-540-85226-1_97, © Springer-Verlag Berlin Heidelberg 2008
194
40 nm
Figure 1. TEM image showing a collection of Pt nanoparticles composed mainly of truncated cubes.
vacuum
H2
O2
5 nm Figure 2. TEM image of the same Pt particle observed under vacuum (on the left), under hydrogen (in the middle) and under oxygen (on the right).
195
EELS in monochromated and Cs probe corrected TEM: a relevant alternative to soft-XAS in synchrotron to investigate nanostructures M. Cheynet1, S. Pokrant2, S. Ersen3. 1. Laboratoire SIMaP 1130 rue de la Piscine BP75 Saint Martin d’Hères 38042 France. 2. Carl Zeiss NTS GmbH, 73447 Oberkochen, Germany. 3. TEM group, Forschungszentrum Caesar, 53175 Bonn, Germany. [email protected] Keywords: Cs probe corrected TEM, Monochromator, core and low loss spectra of TiO2 anatase.
Up to recently, soft-X-Ray Absorption Spectroscopy (SXAS) performed in the context of a 3rd generation Synchrotron Radiation Source (SRS), was the natural experimental way to probe element partial density of empty electronic states. Thanks to the coupling to high resolution monochromator, energy resolution around 0.1 eV is currently achieved in XAS spectra, in an energy range as low as 100-1000 eV. Nowadays, with the development of monochromator and electron probe corrector, 0.1eV energy resolution with beam current ten times higher than in traditional machines can also be obtained in the context of Transmission Electron Microscopes. Thus, EELS in monochromated and Cs probe-corrected FEG-TEM is becoming a reliable alternative to soft-XAS. It is even becoming one of the most relevant tools to investigate nanostructures, because of the sub-nanometer spatial resolution achieved in FEG-TEM. In this work, we report on EELS (core-loss and low-loss) experiments performed using the “CRISP” (i.e. a ZEISS Libra200 Field Emission Gun TEM fitted with a monochromator and a Cs probe corrector, a High Angle Annular Dark Field detector (HAADF) and equipped with a 2nd order corrected Omega filter and a Gatan camera) to investigate TiO2 nano-particles. In this instrumental context, EELS is a simple and fast way to get access to structural information with energy resolution below 0.2 eV and spatial resolution below 1nm. This analytical method works especially well in compounds containing d electrons, as for transition elements based compounds. In these cases, the L2,3-edge is very sharp and strongly influenced by crystal field effects, hence the L2,3-edge ELNES structures are specific for a given crystal structure. In the particular case of TiO2, it is well known that several polymorphic forms exist at ambient conditions. The tetragonal rutile and anatase are the most common phases. As expected, several studies, using soft-XAS in synchrotron radiation [1][2][3] have demonstrated that the Ti-L2,3 edge fine structures are specific for each one of these phases. EELS in conventional TEM have also allowed discriminating these two structures; however the energy resolution is too low to allow resolving all the energy transitions observed in XAS spectra or predicted from calculations. In the first part, we will show the benefits obtained by the coupling of a FEG-TEM to a monochromator and a Cs probe corrector. For this purpose the Zero-Loss peak recorded in vacuum with monochromator “on” and “off” are compared. Then, the Ti-
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 195–196, DOI: 10.1007/978-3-540-85226-1_98, © Springer-Verlag Berlin Heidelberg 2008
196
L2,3 edge recorded on TiO2 nano-particles with the monochromated (on and off) and Cs probe corrected system are compared to spectra recorded with a “conventional” TEM [4][5] (fig.1). In the second part, the EELS Ti-L2,3 spectrum, recorded on TiO2 nano-particles, using illumination angle α=16mrad, collection angle β= 5mrad, dispersion=0.02eV and probe size of 0.19nm measured in Si, are compared to anatase TiO2 synchrotron soft-XAS spectra published in the literature (figure 2). From the analysis of the full width at half maximum (FWHM) of the Ti-L3 t2g band, we show that the energy resolution achieved in monochromated and Cs probe corrected spectra is as high as in XAS spectra (table 1). In the last part, we present the low-loss spectra recorded on TiO2 nano-particles and compare them to low-loss spectra acquired using a 0.75 eV energy resolution machine and to calculated low-loss spectra [6].
Figure 1. Ti-L2,3 edge recorded from anatase using a Philips CM30 (dotted line) and a Zeiss-CRISP monochromator “On” and “Off” (full line).
Figure 2. Ti-L2,3 edge recorded from anatase: XAS spectrum (dotted line); monochromated and Cs probe corrected EELS spectrum (full line).
Table 1. Comparison of the Full Width at Half Maximum of the Ti-L3 t2g band in different instrumental environment (XAS in Synchrotron or EELS in TEM) Experimental configuration FWHM of the L3 t2g edge CRISP (TEM+mono+ Cs probe)Re : 0.23 eV 0.40 eV this work CM30 GIF 2000 (Re : 0.75 eV) 1.20 eV ref .5 XAS (beam line 8 Berkeley) Re : 0.2 eV 0.39 eV ref.1 VG (Cold FEG-TEM) Re : 0.5 eV 0.72 eV ref.4 XAS (beamline22 MAX LAB Lund Sweden) Re 0.3eV 0.48 eV ref.2 XAS (SRRC-HSGM- Taipei, Taiwan) Re 0.2-03 eV 0.46 eV ref.3 1. 2. 3. 4. 5. 6.
S.O. Kucheyev et al., Phys. Rev. B. 69 (2004) 245102. R. Ruus et al., Sol. Stat. Com. 104, n°4, (1997) 199. Y. Hwu, Y.D Yao, N.F. Chen, C.Y. Tung, H.M. Lin, Nanostructured Mat., 9 (1997) 355. R. Brydson et al, J. Phys. : Conden. Matter, 1 (1989) 797. G. Bertoni et al. Ultramicroscopy 106 (2006) 630. M. Launay, F. Bouchet, P. Moreau, Phys. Rev. B, 69 (2004) 035101.
197
Atomic-resolution Electron Microscopy at Ambient Pressure J.F. Creemer1, S. Helveg2, A.M. Molenbroek2, P.M. Sarro1 and H.W. Zandbergen3 1. DIMES-ECTM, Delft University of Technology, P.O. Box 5053, 2600 GB Delft, The Netherlands 2. Haldor Topsøe A/S, Nymøllevej 55, DK-2800 Kgs. Lyngby, Denmark 3. Kavli Institute of Nanoscience, HREM, Delft University of Technology, P.O. Box 5046, 2600 GA Delft, The Netherlands j [email protected] Keywords: Environmental TEM, ETEM, microelectromechanical systemts, MEMS, gas-solid interactions, nanocrystals, heterogeneous catalysis
High-resolution TEM (HRTEM) is a powerful technique for atomic-scale imaging of nanomaterials that are kept under high vacuum conditions. However, the technique is also used in in situ studies of gas-solid interactions; an application generally referred to as environmental TEM (ETEM). ETEM at the atomic-scale is very demanding because the gas atoms scatter the electron beam and thereby degrade the resolution. A key requirement for ETEM is therefore that the number of gas atoms along the path of the electron beam is limited. The limitation of the number of gas atoms is usually reached by confining the gas around the solid specimen. The confinement is attained by two types of instruments: differentially pumped vacuum systems and windowed cells [1]. Recently, both instruments have provided images showing atomic lattice fringes with spacing smaller than 0.2-0.3 nm. In these experiments the solid specimens were exposed to gasses at pressures up to about 10 mbar and temperatures up to 900 ºC; see e.g. [2-4]. This atomic-resolution ETEM has led to significant new insights into the mechanisms of gas-solid reactions in a variety of nanostructured materials, such as heterogeneous catalysts [2-4]. It is, however, important that the new insights are applied with caution. The gas pressures of a few millibars are much lower than the ambient pressures of 1 bar and more in which many nanomaterials find technological application. Because the state and properties of nanomaterials can depend strongly on the gas environment it is therefore desirable to have an instrument for atomic-scale reaction imaging at higher pressures for research on applied nanomaterials [5]. Here we report on a novel nanoreactor that enables atomic-resolution ETEM of nanomaterials during exposure to heat and gases at ambient pressure [6]. This is achieved by miniaturizing the gas volume and heater into a microelectromechanical system (MEMS). It fits into the tip of a dedicated sample holder that can be used in a normal CM microscope of Philips/FEI. The performance of the nanoreactor was demonstrated by the in situ studies of a Cu/ZnO catalyst for methanol synthesis. The nanoreactor allowed for the direct observation of nanocrystal growth and mobility on a sub-second time scale during heating to 500 ºC and exposure to 1.2 bar of H2. In the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 197–198, DOI: 10.1007/978-3-540-85226-1_99, © Springer-Verlag Berlin Heidelberg 2008
198
same environment, HRTEM images showed atomic lattice fringes in the Cu nanocrystals with spacings that demonstrate a spatial resolution of 0.18 nm. We anticipate that the nanoreactor will generate new insights into a variety functional nanomaterials and the way they interact with ambient environments. 1. 2. 3. 4. 5. 6. 7.
E.P. Bulter, K.F. Hale, Dynamic experiments in the electron microscope, Practical Methods in Electron Microscopy, vol. 9, Nthe Holland, Amsterdam (1981). E.D. Boyes, P.L. Gai, Ultramicroscopy 67 (1997), p. 219 S. Giorgio, S. Sao Joao, S. Nitsche, D. Chaudanson, G Sitja and C.R. Henry, Ultramicroscopy 106 (2006), p. 503. P.L. Hansen, S. Helveg and A.K. Datye, Adv. Catal. 50 (2006), p. 77. N.I. Jaeger, Science 293 (2001), p. 1601. J.F. Creemer, S. Helveg, G.H. Hoveling, S. Ullmann, A.M. Molenbroek, P.M. Sarro and H.W. Zandbergen, accepted to Ultramicroscopy (2008). This work is supported by STW, applied science foundation of NWO and the Ministry of Economic Affairs with financial contributions from FEI Company, Haldor Topsøe A/S, and the European ESTEEM project.
199
Development of a system for TEM/STEM investigation of air-sensitive materials: Preliminary results on CeO2 reduction behaviour J.J. Delgado, M. López-Haro, J.D. López-Castro, J.A. Pérez-Omil, S. Trasobares and J.J. Calvino Departamento de Ciencia de Materiales e Ingeniería Metalúrgica y Quimica Inorgánica. Facultad de Ciencias. University of Cadiz. Apdo. 40. 11510 Puerto Real (Cádiz). SPAIN [email protected] Keywords: air sensitive materials, STEM, CeO2 reduction
High Resolution Transmission Electron Microscopy is a powerful tool for advanced nanostructured catalyst characterization [1]. The use of structural as well as analytical techniques (HREM, ED,STEM-HAADF, EELS or EDX) has been crucial to perform a thorough structural, morphological and compositional study of a wide variety of materials at the nanometric scale. However, in the case of catalysts characterization, the study of the chemical environment/sample interaction is conventionally carried out by pre-treating the sample in a conventional reactor, depositing the sample on a grid and finally transferring it into the TEM equipment under air. Some of these materials, like pre-reduced oxides, are oxygen sensitive and the previously mentioned experimental design does not allow to observe the material in its native state. One of the most appealing approaches to solve this problem is the use of dedicated environmental transmission electron microscopes (ETEM) which allow in-situ characterization [2]. Nevertheless, although ETEM allow a live monitoring of the dynamics of gas–solid interactions, the currently available in-situ stages can only operate at pressure values in the millibar range. Thus, a challenging gap to be addressed is to study the gas–solid interactions under more realistic operating conditions. The use of an environmental reaction cell specific for an anaerobic-transfer TEM holder is an alternative approach that allows carrying out the pre-treatment of the sample under more realistic conditions and subsequently transferring it to the TEM, under conditions which prevent any ulterior sample modification. Although the dynamic aspects of the gas-solid interactions are lost in this alternative approach, the characterization of those structural and compositional features which are induced by realistic thermo-chemical treatments, which could be lost by interaction with air components but which are not reversed by evacuation or cooling, can be investigated. Here we present details about the development of a system for TEM/STEM investigation of air-sensitive materials which allow treatments under flow conditions at high pressure as well as the preliminary results we have obtained in the study of CeO2 and Rh/CeO2 reduction/oxidation behaviour. Samples of these two materials were heated at different temperatures (200-800ºC) under vacuum as well as under flowing inert and H2/Ar mixture at atmospheric pressure. After evacuation of the reaction cell,
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 199–200, DOI: 10.1007/978-3-540-85226-1_100, © Springer-Verlag Berlin Heidelberg 2008
200
the samples were transferred into the TEM under anaerobic conditions to study the structural accommodation of the oxygen deficiency induced by the reduction treatments. We should recall that for CeO2, as well as for some other higher rare earth oxides with fluorite structure, an homologous series of reduced phases, LnnO2n-2m, is known. The members of these series are just superstructures of the fluorite cell characteristic of the dioxide, generated by ordering of oxygen vacancies. In the case of CeO2 experimental evidences from neutron diffraction as well as electron microscopy has allowed detecting the presence of some members of this series in reduced samples [3]. Figure 1 shows some HREM and Digital Diffraction Patterns observed in the Rh/CeO2 material after different pre-treatments. The DDPs contain spots which don’t correspond to the fluorite structure but that can be easily explained by considering the formation of the so-called π (CeO1 875) and β(3) (CeO1 833) phases of the homologous series. It should be pointed out that reduced ceria re-oxidises quite fast and thoroughly even at room temperature. Thus, the identification of patches of these reduced phases demonstrates that the equipment is working properly and that allows creating and preserving the material in a reduced state, being thus suitable to investigate air-sensitive materials. Though this is an aspect that deserves a more detailed experimental work, it is also worth emphasizing that these two phases, π and β(3), have not been detected in reduced samples of CeO2. This experimental fact points out the interest of performing detailed TEM studies with samples prepared under well controlled and more realistic conditions. 1. 2. 3.
P.L. Gai and J.J. Calvino; Annu. Rev. Mater. Res. 35 (2005) 465-504; Boyes, E.D. and P.L. Gai. Ultramicroscopy. 67(1-4): p. 219-232 (1997) C. López-Cartes, J.A. Pérez-Omil, J.J. Calvino, J.M. Pintado, L. Eyring y Z.C. Kang. Ultramicroscopy. 80(1): p. 19-39 (1999)
002
022
[401]π
Figure 1. High-resolution micrographs of a Rh/CeO2 sample after pre-treatment under H2-Ar (left) and vacuum (right) at 800 ºC and subsequent transfer to the microscope under anaerobic conditions. Digital diffractograms are included.
201
Characterization of two new zeolites by combining Electron Microscopy and X-Ray Powder Diffraction analyses E. Di Paola, E. Montanari, S. Zanardi and A. Carati Eni S.p.A., Refining & Marketing Division, San Donato Milanese Research Center, Via F. Maritano 26, I-20097 San Donato Milanese (MI) Italy [email protected] Keywords: zeolite, XRPD, SEM, HRTEM
During exploratory zeolite crystallization experiments performed in our labs, two new materials, named ERS-13 and ERS-14, were synthesized. They were obtained in the frame of a wide activity focused on the use of diquaternary alkylammonium dications (diquats) of general formula [R3N-(CH2)n-NR3]2+ as structure directing agents (SDAs). In particular ERS-13 and ERS-14 were obtained by hydrothermal method using N,N’-tetramethylen-bis-(N-methylpiperidinium) dyhydroxide as SDA. The two products were widely characterized by means of X-Ray Powder Diffraction (XRPD), 29Si Nuclear Magnetic Resonance (NMR) [1], Scanning Electron Microscopy (SEM) [1] and High Resolution Electron Transmission Microscopy (HRTEM). ERS-13 crystallizes as thin plates arranged in form of “desert rose”-like aggregates. The XRPD pattern and the 29Si NMR analysis suggested a partial similarity of ERS-13 with the layered material ITQ-8 [2] and, like this one, it undergoes complete breakdown upon calcination at 550°C. The result of HRTEM characterization is shown in Figure 1; work is in progress in order to determine the crystal structure of this material. ERS-14 showed a XRPD pattern similar to that already reported for the zeolite ITQ10 [1], which was claimed to belong to the zeolite beta family [2,3]. However, a new, weak peak at 2θ = 3.7° (λ = 1.54178 Å), related to a periodicity of 23.6 Å, was found in the XRPD pattern of ERS-14. This peak was not observed in the pattern of ITQ-10 and never reported for the zeolite beta family. In agreement with the XRPD analysis, the Selected Area Electron Diffraction showed a periodicity of 47 Å, which is double with respect to that found by XRPD. On the basis of the HRTEM images, this periodicity was attributed to the formation of the polytype C of zeolite beta [3] between not well defined zones (Figure 2). 1. 2. 3.
The authors thank Elisabetta Previde Massara for SEM characterization and Wallace O’Neil Parker Jr. for NMR analyses. M.J. Diaz-Cabanas, M.A. Camblor, Z. Liu, T. Ohsina and O. Terasaki, J. Mater. Chem. 12 (2002), p. 249. J.M. Newsam, M.M.J. Treacy, W.T. Koetsier and C.B. de Gruyter, Proc. R. Soc. London A 420 (1988), p. 375
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 201–202, DOI: 10.1007/978-3-540-85226-1_101, © Springer-Verlag Berlin Heidelberg 2008
202
Figure 1. HRTEM micrograph (200 kV) of ERS-13 and Electron Diffraction pattern from selected area.
Figure 2. HRTEM micrograph (200 kV) of an ERS-14 crystal; the periodic formation of the polytype C of zeolite beta between not well defined zones is shown.
203
Electron beam-induced effects on copper nanoparticles: coarsening and generation of twins D. Díaz-Droguett1, V. Fuenzalida1 and G. Solórzano2 1. Universidad de Chile, Av. Almirante Blanco Encalada 2008, Santiago, Chile 2. PUC-Rio, Rua Marquês de São Vicente 225, Gávea, Rio de Janeiro, Brazil [email protected] Keywords: nanoparticles, copper, twin
This work reports on the in situ-generation of twins due to the incidence of electron beams on copper nanoparticles when they are investigated under transmission electron microscopy (TEM). Copper nanoparticles were synthesized by means of the inert gas condensation (IGC) method, using hydrogen as carrier gas. The IGC method involves the physical evaporation of a material in the presence of a carrier gas at a pressure around 100 Pa [1]. At this pressure the mean free path is in the submillimeter range and the evaporated material cools down by colliding with the carrier gas molecules in its path, leading to nanoclusters collected onto a cold surface. The size of the nanoclusters depends on the evaporated material, the carrier gas and it pressure; lighter gases lead to the production of smaller particles [1,2]. In this research the IGC method was used to generate copper nanoparticles in hydrogen at pressures between 100 and 1200 Pa and evaporation source temperatures in the range from 1320°C to 1730°C. X-ray powder diffraction (XRD) revealed particles of inhomogeneous composition, with metallic copper, Cu2O and CuO in variable amounts. This is attributed to the oxidation of the copper nanoparticles due to the air exposition after venting the chamber to remove the material from the collector surface. The oxidation state of the surface of the particles was corroborated by X-ray photoelectron spectroscopy (XPS). The morphology and size of the particles was analysed by TEM and their cristallinity by selected area electron diffraction (SAED) patterns. Figure 1 shows a bright field and dark field TEM image with agglomerated copper powder on the grid. At higher magnification faceted particles of about 15 nm were observed. These nanoparticles were not stable under electron irradiation: the thermal stimulus caused the coarsening of the nanoparticles and formation of new ones with twins. Since the particles do not exhibit additional structural changes after longer irradiation, we believe that the twins confer stability to the nanoparticles. The sequential changes at different irradiation times are shown in Figure 2. 1. 2. 3.
C. Granqvist, R. Buhrman, J. Apl. Phy.; vol 47, N.5 (1976). M. Turker, Mat. Sci. and Eng. A 367 (2004) 74-81 This work was partially financed by the Chilean government under grant FONDECYT 1070789. D.Díaz-Droguett acknowledges a doctoral fellowship from CONICYT.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 203–204, DOI: 10.1007/978-3-540-85226-1_102, © Springer-Verlag Berlin Heidelberg 2008
204
Figure 1. TEM images showing the agglomerated copper powder on the grid. (a) bright field. (b) dark field.
Figure 2. (a), (b) (c), (d) (e), (f), (g) and (h) are TEM images showing the sequential changes at different irradiation times: coarsening of two copper nanoparticles and formation of twins.
205
Role of the catalyst and substrate in nucleation and growth of Single Wall Carbon Nanotubes in HFCVD M.-F. Fiawoo1, N. Brun2, A.-M Bonnot3, O. Stephan2 , J. Thibault4 and A. Loiseau1 1. LEM, ONERA/CNRS UMR104, 92322 Châtillon, France 2. LPS, CNRS UMR 8502, Université Paris Sud, 91405 Orsay, France 3. Institut Louis Néel, CNRS , 25 avenue des Martyrs, 38042 Grenoble, France 4. TECSEN, CNRS UMR622, Université Paul Cézanne Aix-Marseille III, 13397 Marseille, France fiawoo@onera fr Keywords: carbon nanotubes, nuclei, growth, catalyst
Nowadays many kinds of CVD (Chemical Vapour Deposition) processes manage to produce bundles and isolated SWCNTs (single wall carbon nanotubes) from supported catalytic particles. In order to understand the growth mechanism of these tubes and the role of the catalyst in these processes, as it had already been done for the high temperature syntheses [1, 2], we have undertaken a systematic study by TEM (Transmission Electron Microscopy) of the nanotubes and of their relationships with catalytic particles at different stages of their growth. With this aim, nanotubes were grown by HFCVD (Hot Filament Chemical Vapour Deposition) and the synthesis stopped at different times from 40 s to 50 mn. Catalytic particles were prepared in situ by heating, under a hydrogen atmosphere, a few monolayers of cobalt deposited on silica substrates. These substrates have been specially manufactured, prior to the synthesis, in order to make possible the observation of the nanotubes and particles along the synthesis process (Figure 1) [3]. Our observations demonstrate that, whatever the particle size, ranging from 1.4 to 5 nm, nanotubes nucleate either parallel or perpendicularly to the surface of catalyst particles, with in the latter case, no correlation between the diameters of the tubes and the particles (Figure 1). Surprisingly, tube nuclei are observed all along the synthesis but the perpendicular nucleation mode increases with time. This suggests that corresponding nuclei do not evolve towards nanotubes but are frozen. Thanks to electron diffraction and electron energy loss spectroscopy analyses of the particles, we have shown that metal particles chemically react with silica membranes and progressively transform into a silicide (Figure 2). This reaction is presumed to lead to a deactivation of the catalyst and to the abortion of the nanotube growth. The selective death of a kind of nucleus therefore suggests that different kinetics of growth occur depending on the nucleation mode. This conclusion is supported by the distribution in diameter of the tubes, which is found to be much narrower than that of the nuclei. This lack of correlation suggests that some structural rearrangements take place, before the settlement of the final structure of the tube, which depends on the nucleation mode. As a consequence, different growth kinetics occur which compete with the kinetics of metal – membrane reactions leading to the death of the slowest growing nuclei. Finally our
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 205–206, DOI: 10.1007/978-3-540-85226-1_103, © Springer-Verlag Berlin Heidelberg 2008
206
results also suggest that helicity of the nanotubes is not settled at the nucleation stage, but later on, during the structural rearrangements of the nuclei. 1. 2. 3.
J. Gavillet et al., P.R.L. 87 (2001), p. 275504-1. A. Loiseau al., C. R. Physique, 4 (2003), p. 975-991. M.-F. Fiawoo et al, JNN submitted (2008)
Figure 1. (a): Suspended SWNTs (b): Isolated carbon nanotube. (c): a nucleus with the graphen sheet parallel to tangent of the cobalt nanoparticle. (d): a nucleus with the graphen sheet perpendicular to the tangent of the cobalt nanoparticle, the arrow is pointing out the end of the nucleus.
Figure 2. The EELS spectra shows the silicon edge showing the onset for cobalt silicide in the dotted square and the silica spectra in black. Bellow, HADF image of a nanotube and cobalt nanoparticles on a silica membrane and chemical maps of Co, Si, O edges and the Si onset.
207
PEMFC degradation phenomena studied by electron microscopy L. Guetaz1, B. Vion-Dury1 and S. Escribano1 1. CEA – LITEN, LCPEM, 17 rue des Martyrs, 38048 Grenoble cedex 9, France laure.guetaz@cea fr Keywords: PEMFC, degradation, electrocatalyst
Proton-exchange membrane fuel cells (PEMFC) that combine hydrogen and oxygen to produce electricity are attractive zero emission power sources for nomad and stationary applications. The heart of PEMFC is the membrane electrode assembly (MEA). It consists of a proton exchange membrane coated on both side with active layers (AL), where electrochemical reactions take place, and with gas diffusion layers. Fuel cell performance is largely controlled by the AL microstructure composed of nanometer-scale metallic electrocatalysts supported on black carbon surrounding by recast ionomer. Today, significant obstacles to the commercialization of PEMFC result from a large degradation of the performances upon operation. It has been evidence that this performance degradation is due to the degradations of the AL components such as catalyst particle coarsening or carbon support corrosion. However, the relative contribution of each component to PEMFC performance loss and the mechanisms by which the different components are degraded are still largely unknown. For a better understanding, it is therefore necessary to analyse in detail the degradation of each AL constituents. We compare in this study MEA microstructure before and after electrochemical aging. Different SEM and TEM techniques are used for this purpose, depending on the microstructural parameter to characterize: -
-
-
Electrocatalysts: the evolution of the catalyst distribution resulting from coarsening mechanism has been studied using conventional TEM or STEM modes. When the electrocatalysts are bimetallic (Pt-M) nanoparticles, HRTEM, HAADF-HRSTEM and EDX microanalysis have been performed in order to observe the nanoparticle structural and chemical composition changes. Carbon support and re-cast ionomer degradation: The HRTEM images of AL (figure 1a) clearly show the catalyst carbon support surrounding by a few nanometer thick ionomer layer. This thin ionomer layer can also be imaged using HAADF-STEM mode (figure 1b). Porosity: the AL porosity is another crucial parameter that provides gas access to the catalyst site. The 2D porosity can be imaged by FEG-SEM in STEM mode (figure 2). Electron tomography is required for a better knowledge of the porosity in three dimensions.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 207–208, DOI: 10.1007/978-3-540-85226-1_104, © Springer-Verlag Berlin Heidelberg 2008
208
a)
b)
Figure 1. Catalyst carbon support surrounding by a few nm thick ionomer layer. a) HRTEM image. b) HAADF-STEM image.
Figure 2. STEM image showing the porosity of the active layer in projection. Electron tomography is required for a better understanding of the porosity in three dimensions.
209
TEM investigation of magnetite nanoparticles for biomedical applications S. Gustafsson1, A. Fornara2, F. Ye2, K. Petersson3, C. Johansson3, M. Muhammed2 and E. Olsson1 1. Department of Applied Physics, Chalmers University of Technology, SE-412 96 Göteborg, Sweden 2. Division of Functional Materials, Royal Institute of Technology (KTH), SE-164 40 Kista, Sweden 3. Imego AB, Arvid Hedvalls Backe 4, SE-411 33 Göteborg, Sweden [email protected] Keywords: TEM, magnetite
Magnetic nanoparticles (MNP) are interesting for use in a wide range of biomedical applications including targeted drug delivery, immunoassays, hyperthermia and magnetic resonance imaging (MRI) [1]. The performance of MNP in such applications is dependent on the particle properties which are governed by the particle size, shape and chemistry. This abstract presents a transmission electron microscopy (TEM) study of the nanoscale structure and chemistry of magnetite MNP. The analysis was performed using a Philips CM200 TEM equipped with a field emission gun and operating at 200 kV. Energy dispersive X-ray (EDX) analysis was performed using a Link ISIS system and energy filtered TEM (EFTEM) was performed using a Gatan Imaging Filter (GIF) attached to the microscope. Specimens for TEM were prepared by placing a drop of the ferro fluid on a holey carbon coated copper grid. Figure 1 shows an overview of the magnetic nanoparticles and the corresponding size distribution, as calculated from data from at least 300 particles. The mean particle diameter is 20 nm and the size distribution can be considered as narrow. It can be modelled with a normal distribution. Selected area diffraction in the TEM confirms that the structure of the particles is that of magnetite. EDX analysis also shows that the Fe:O ratio is close to that expected for stoichiometric magnetite. EFTEM imaging of the particles indicates the uniform distribution of iron and oxygen (Figure 2). High resolution TEM (Figure 3) shows that most particles are single crystals. These features are desirable from an application point of view. The particles have sizes just above the superparamagnetic limit which means that they are well suited for specific immunoassay applications [2]. 1. 2.
U. Jeong, X. Teng, Y. Wang, H. Yang and Y. Xia, Advanced Materials 19 (2007), p. 33. A. Prieto Astalan, F. Ahrentorp, C. Johansson, K. Larsson, A. Krozer, Biosensors and Bioelectronics 19 (2004), p. 945.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 209–210, DOI: 10.1007/978-3-540-85226-1_105, © Springer-Verlag Berlin Heidelberg 2008
210
(a)
(b)
Figure 1. (a) TEM micrograph showing the magnetite nanoparticles. (b) The size distribution of the magnetite nanoparticles.
(a)
(b)
(c)
Figure 2. (a) Bright field image (b) Fe jump ratio image (c) O jump ratio image of magnetite nanoparticles.
Figure 3. High resolution TEM image of a magnetite particle.
211
Catalytic soot oxidation studied by Environmental Transmission Electron Microscopy S.B. Simonsen1, S. Dahl1, E. Johnson and S. Helveg1 1. Haldor Topsøe A/S, Nymøllevej 55, DK-2800 Kgs. Lyngby, Denmark 2. Nano-Science Center, Niels Bohr Institute, University of Copenhagen, Denmark [email protected] Keywords: ETEM, catalysis, soot oxidation, diesel engine, emission control
At present, the awareness of soot abatement in the exhaust from diesel engines is increasing due to new environmental legislation for exhaust specifications. An attractive approach for effective soot removal includes the introduction of filters on the dieseldriven vehicles and the functionalization of the filters for catalytic soot oxidation by ceria-based materials. Although it is generally accepted that the redox properties of ceria are crucial to the catalytic effect, the detailed reaction mechanism and the location of the catalytic active sites are still matters of debate. In this contribution we present an Environmental Transmission Electron Microscopy (ETEM) study of ceria-catalyzed soot oxidation related to diesel engine emission control [1]. ETEM has become a powerful tool in heterogeneous catalysis due to its ability to directly monitor catalysts in situ during exposure to reactive gases at elevated temperatures [2]. From time-lapsed ETEM image series of soot particles in contact with a CeO2 catalyst, as illustrated in fig. 1, direct observations at the soot-catalyst interface were obtained during exposure to oxidation conditions and provided mechanistic and kinetic insight into the catalytic oxidation reaction. The results show that the catalytic oxidation reaction involved processes, which were confined to the soot-CeO2 interface region, and that the catalytic reaction surprisingly resulted in motion of soot agglomerates toward the catalyst surface, which acted to re-establish the soot-CeO2 interface in the course of the oxidation process. The observed reaction dynamics was found to be consistent with observations from ex situ oxidation experiments and quantitatively in good agreement with previous kinetic measurements. 1. 2.
S.B. Simonsen, S. Dahl, E. Johnson and S. Helveg, J. Catal. 255 (2008), p. 1. P.L. Hansen, S. Helveg and A.K. Datye, Adv. Catal. 50 (2006), p. 77.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 211–212, DOI: 10.1007/978-3-540-85226-1_106, © Springer-Verlag Berlin Heidelberg 2008
212
a
b
c
CeO2 soot
Figure 1. Time-lapsed ETEM images of soot in contact with a CeO2 catalyst during the exposure to 2mbar O2 at 550ºC. The time interval between the images is ~2min. Scale bar , 90nm. The figure adapted from [1].
213
Surface and interface structure of ceria supported ruthenium J.C. Hernandez1, S. Trasobares1, J.M. Gatica1, D.M. Vidal1, M.A. Cauqui1, J.J. Calvino1, A.B. Hungria1 and J.A. Perez-Omil1 1. Dpto. Cienica de los Materiales, Ingenieria Metalurgica y Quimica Inorganica, Universidad de Cadiz, Campus Rio San Pedro s/n, Puerto Real 11510 (Cadiz), Spain [email protected] Keywords: ruthenium catalysts, ceria mixed oxides, electron microscopy
Noble metals highly dispersed on cerium mixed oxide supports Ce(M)O2-x (M=Zr,Tb) are currently being investigated, not only due to their relationship with the so called Three-Ways Catalysts (TWC) but also because of their potential applications in other catalytic processes related to the hydrogen production or the elimination of organic pollutants in residual waters from different industrial processes [1]. Among these supported noble metals catalysts, Ru containing materials seems to be more stable while at the same time very active and selective in comparison with other supported noble metals [2]. This contribution is aimed at investigating the structural features of a new family of ceria-based catalytic materials with Ru as metallic phase. Specifically, the work has been focused on the study of the chemical and nano-structural changes induced on Ru nanoparticles by reduction treatments in hydrogen at increasing temperatures, within the range 623 K - 1173 K. We report detailed information about the nature of the metallic phase (metallic particle morphology and crystallographic features of its exposed surfaces), of the supports as well as of the possible interactions between both components, for a series of Ru nanoparticles supported on different cerium mixed oxides (Ce0 5Zr0 38Tb0 12O2-x, Ce0 62Zr0 38O2 and Ce0 8Tb0 2O2) using high resolution electron microscopy (HREM), high angle annular dark field (HAADF-STEM) imaging, electron energy loss spectroscopy (EELS) and X-ray analysis (XEDS). HREM studies showed that in the whole range of reduction temperatures the Ru nanoparticles were well faceted with morphology close to a truncated hexagonal pyramid as well as epitaxial relationships between metallic nanoparticles and the oxide supports through Ru(002) || Ce(M)O2-x(-111) and Ru[010] || Ce(M)O2-x[110], Figure 1. XEDS and EELS studies confirmed that Ru did not seem to be affected by decoration layers on top of the metal particles or by the formation of alloys or intermetallic phases even after reduction at the highest temperature (1173K), in contrast to that observed for other noble metals like Rh or Pt supported on the same Ce0 8Tb0 2O2 support [3]. A remarkable feature of the Ru catalysts treated in hydrogen at the highest temperature, 1173K, is the presence of small "pedestals" under some metallic particles. The frequency of appearance of these peculiar nanostructures under the metallic nanoparticles increases with the Tb-content of the oxide support (Ce0 8Tb0 2O2 >> Ce0 50Zr0 38Tb0 12O2 >>> Ce0 62Zr0 38O2). The electron microscopy studies (HREM,
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 213–214, DOI: 10.1007/978-3-540-85226-1_107, © Springer-Verlag Berlin Heidelberg 2008
214
HAADF, XEDS and EELS) of the high-temperature treated catalysts showed that the Ru particles keep the same epitaxial relationship already observed after reduction at low temperature, defined by Ru(002) || Ce0 8Tb0 2O2(1-11) and Ru[-2-10] || Ce0 80Tb0 20O2 [2-11]. Likewise such studies also evidenced that the chemical composition in the pedestals, i.e. in the regions of the oxide close to the metallic nanoparticles, was comparable to that observed in other areas of the support, Figure 2. 1. 2. 3. 4.
D. L. Trimm, Z. I. Onsan, Catalysis Reviews-Science and Engineering 43 (2001), 31. R. Lanza, S.G. Järås and P. Canu, Applied Catalysis A: General 325 (2007), 57. S. Bernal, G. Blanco, J.J. Calvino, C. López-Cartes, J.A. Pérez-Omil, J.M. Gatica, O. Stephan and C. Colliex, Catalysis Letters 76 (3–4) (2001), 385. We acknowledge the financial support from Ministry of Education and Science of Spain (MAT2005-00333) and Junta de Andalucia (FQM334, FQM110). Electron microscopy imaging was carried out in the Central Service of Science and Technology from Universidad de Cadiz.
[010] (002) 61º (002)
61º
(101)
(100)
(101)
(101)
[110] (111)
2 nm Figure 1. HREM image of a Ru(1%)/Ce0 62Zr0 38O2 catalyst reduced under H2 at 1173K. The structural analysis shows an epitaxial relationship between the metallic phase and the support defined by Ru(002) || Ce0 62Zr0 38O2(-111) and Ru[010]|| Ce0 62Zr0 38O2[110]. 1000
800 Ru
Ce
O
600
Tb Tb 400
Ce
pedestal
Ce Tb
O
Cu
Tb
Ce Ce
Tb Tb
200
Cu
particle
Ce Tb
support
Cu
Tb
0 0
2
4
keV
6
8
10
Figure 2. (Left) HREM image of a Ru(1%)/Ce0 8Tb0 2O2 catalyst reduced under H2 at 1173K showing pedestal-like nanostructures. Note the epitaxial relationship between the metallic phase and the support. (Center) XEDS compositional analysis showing similar chemical composition in the pedestal areas and the support. (Right) HREM image showing the distance between the metal and the oxide in the interface.
215
Characterisation of materials with applications in the photocatalytic activation of water N.S. Hondow1, R. Brydson1, Y.H. Chou2 and R.E. Douthwaite2 1. Institute for Materials Research, University of Leeds, Leeds, LS2 9JT, United Kingdom 2. Department of Chemistry, University of York, York, YO10 5DD, United Kingdom n [email protected] Keywords: photocatalyst, TEM, STEM
The requirement for the development of alternative fuel sources is highlighted by the limited supplies of fossil fuels and the environmental impact caused by their extensive use. The conversion of solar energy is a particularly desirable option, with the photocatalytic conversion of water into hydrogen and oxygen representing an attractive source of fuel. An ideal material suitable for this type of reaction has yet to be reported, though several promising developments have been made. An ideal photocatalyst would exhibit certain characteristics, such as long term stability, optimum absorption of the solar spectrum, and the ability to oxidise and reduce water to O2 and H2 respectively. Stable oxide semiconductors have shown the best results, with the possibility of manipulating the valence and conduction bands of the materials through alteration of the composition and structure allowing the required redox reactions. However, the materials developed at present generally have an overall low efficiency as they only utilise the high energy UV periphery of the solar spectrum [1]. This therefore creates the need for either the development of new materials, or the further improvement of these known systems. In either case, the application of alternative synthetic methods may lead to the formation of new phases and novel materials. One such synthetic route currently being investigated is that of using microwave-induced plasma promoted dielectric heating [2]. Materials currently being made include titanates, niobates and tantalates. The morphology and crystallinity of the samples can directly affect the performance of the materials as photocatalysts. It is important that sites for the oxidation and reduction reactions are separated so as to prevent recombination. The morphology of the materials has been examined by field emission SEM and the crystalline structure of the materials has been confirmed using conventional high resolution phase contrast TEM and selected area diffraction. This has been examined at several points throughout the catalyst development, including before and after catalytic testing, enabling observations as to the stability of the materials. Attempts to increase the catalytic performance has led to the introduction of further elements into the systems being investigated, with particular interest in the formation of metal or nitrogen/oxynitride rich surface regions [3,4]. The key factors in how these materials will perform as photocatalysts for the splitting of water include the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 215–216, DOI: 10.1007/978-3-540-85226-1_108, © Springer-Verlag Berlin Heidelberg 2008
216
distribution and composition of these added particles. This has been analysed by high angle annular dark field STEM imaging in combination with EDX mapping. Initial studies have found that some of the conditions the materials are subjected to leads to phase separation of the metals present, rather than the desired surface doping (Figure 1). Further elemental composition, including lighter elements, has also been determined using EELS, and supporting chemical bonding information has been obtained by the surface sensitive technique XPS. 1. 2. 3. 4.
A. Kudo, H. Kato and I. Tsuji, Chemistry Letters 33 (2004), p. 1534. R.E. Douthwaite, Dalton Transactions (2007), p 1002. A. Kudo, R. Niishiro, A. Iwase and H. Kato, Chemical Physics 339 (2007), p 104. Y. Lee, H. Terashima, Y. Shimodaira, K. Teramura, M., Hara, H. Kobayashi, K. Domen and M. Yashima, Journal of Physical Chemistry C 111 (2007), p. 1042.
Figure 1. High angle annular dark field STEM image (left) and EDX maps (right) of NiTa2O6 after attempts at nitrogen doping by reduction in ammonia at 750 oC. EDX maps of Ni (top right) and Ta (bottom right) show that phase separation of the metals has occurred in some particles.
217
Complementary EM study on highly active nanodendritic Raney-type Ni catalysts with hierarchical build-up U. Hörmann, U. Kaiser1, N. Adkins2, R. Wunderlich3, A. Minkow3, H. Fecht3, H. Schils3, T. Scherer4 and H. Blumtritt5 1. Ulm University, Electron Microscopy Group of Materials Science, Albert-Einstein-Allee 11, 89081 Ulm, FRG 2. Ceram, Queens Road, Penkhull, Stoke-on-Trent, ST4 7LQ, Great Britain 3. Ulm University, Institute of Micro- and Nanomaterials, Albert-Einstein-Allee 47, 89081 Ulm, FRG 4. Forschungszentrum Karlsruhe, Institute of Nanotechnology, PO Box 3640, 76021 Karlsruhe, FRG 5. Max-Planck-Institut für Mikrostrukturphysik, Weinberg 2, 06120 Halle/Saale, FRG [email protected] Keywords: Raney-type Ni, dendrites, structure, Cs-corrected HRTEM, gas atomisation, slicing view
Nanostructured Raney-type Ni catalysts have been used in industry since the 1920s for the production of a wide range of chemicals. [1] In the EU supported project IMPRESS it has been shown that by using gas atomisation processing high surface area particles with significantly increased catalytic activity in hydrogenation reactions can be produced. [2,3] Structural investigations with complementary methods of electron microscopy in combination with X-ray powder diffractometry have enabled the link between processing, structure and catalytic activity to be explored. [4] Raney-type Ni catalysts were produced from alloy powder prepared by gas atomisation. After activation by leaching with NaOHaq and prior to the structural investigations the samples were passivated with oxygen. Size selected microparticles of ca. 100 µm size, grown from different melt compositions were chosen for this study. The microstructure of the samples was characterised in 2D by light microscopy and by SEM, see Fig. 1, and SEM EDX mappings. The nanostructure was investigated with HRTEM and Energy filtered TEM for elemental mappings (Ni, Al) using a Cs-corrected FEI 80-300 Titan microscope operated at 300kV. The use of a dual-beam FIB SEM for sample preparation allowed the investigation of one particular nanodendrite on different scales, first within the microparticle by SEM and hereafter as a single cut lamella in the TEM. In order to correlate the local structure with integral measurements, X-ray powder diffractometry was also carried out. The 3D interconnection of the nanodendrites, which build up the whole particle was imaged with slicing view by using a FIB SEM. The resulting porous particles were found to be built-up of nanodendrites. The thickness of the dendrites decreases with increasing Al content. The samples with the finest dendrites were obtained from Ni-75%Al alloy powder, i.e. from an alloy with a higher Al content than the one which is used to produce the standard commercial catalysts. The dendrites consist of two adjacent phases, from which one after leaching and passivation is transformed into NiO. This phase is located at the dendrite tips, and S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 217–218, DOI: 10.1007/978-3-540-85226-1_109, © Springer-Verlag Berlin Heidelberg 2008
218
might offer the reactive sites for the catalytic reaction. The complex structure was characterised by Cs-corrected HRTEM. On the mesoscale it shows a polycrystalline framework structure with filled mesopores. The nanocrystals within the mesopores clearly reveal texture. The outer surface of the dendrite tips shows nanosteps, which increase significantly the surface area provided for the catalytic reaction, see Fig. 2. 1. 2. 3. 4.
M. Raney: US patent 1563587 (1925) A.M. Mullis, N.J. Adkins, Z. Huang, R.F. Cochrane, Proc. 3rd International Conference on Spray Deposition & Melt Atomization, 2006, Bremen, Germany, CD proceedings F. Devred et al., to be published. U. Hörmann, U. Kaiser, N.J.E. Adkins, R. Wunderlich, A. Minkow, H. Fecht, H. Schils, F. Devred, B. Nieuwenhuys, H. Blumtritt, submitted to 9th International Conference on Nanostructured Materials, Nano 2008, Rio de Janeiro, Brazil (2008)
Figure 1. Left: Light microscopy image of a microparticle from the 75 – 106 µm size fraction with a high inner porosity due to the nanodendritic structure. Right: SEM image of a single dendrite with capped tips (light grey), see arrows.
Figure 2. Left: Dark field micrograph of the interface between the caps and the dendrite backbone. Right: Cs-corrected energy-filtered HRTEM micrograph of the mesopores at the outer rim of the capped dendrite tips, showing the pores and the surface steps.
219
Structural properties of sol-gel synthesized Li+-doped titania nanowhisker arrays U. Hörmann1, J. Geserick2, S. Selve1, U. Kaiser1, and N. Hüsing2 1. Ulm University, Electron Microscopy Group of Materials Science, Albert-Einstein-Allee 11, 89081 Ulm, FRG 2. Ulm University, Institute of Inorganic Chemistry I, Albert-Einstein-Allee 11, 89081 Ulm, FRG [email protected] Keywords: titania, anatase, rutile, nanowhiskers, mesoporous material, HRTEM, sol-gel synthesis
Nanostructured titania is of particular interest for applications in photo-catalysis due to its high catalytic activity. Moreover, these structures are of particular interest for many applications due to their electronic properties, e.g. anti-reflection layers, sensors, vacuum microelectronics. The band gap of the nanoscaled semiconducting anatase is size dependent. The band gap increases in the size range of 15 nm to 3.9 eV [1], compared to the bulk value of 3.2 eV [2], suggesting already a quantum confinement effect. Nanowhiskers, grown in even smaller dimensions as in this study are prospective candidates for showing a transition to the quantum confinement effect. Sol-gel synthesis of mesoporous oxides relies on the self-assembly of the structure directing agents, the surfactants which rule the solidification or crystallisation of the inorganic oxide. Mesoporous ordered solids produced by sol-gel processing are e.g. monolithic SBA-15 type silica networks or the highly catalytically active mesoporous titania powders. In this study titania nanowhisker arrays with a high surface area were produced. Anatase nanowhiskers were grown in a sol-gel process [3] using ethylene glycol modified titanium(IV) (EGMT) as the titania precursor and Lithiumdodecyl sulphate (LDS) as a structure directing agent. The LDS simultaneously delivers the Li+ as a dopant. After synthesis the samples were dried and calcined in order to remove the surfactant. The samples were characterised by X-ray powder-diffractometry. The dried samples were found to consist of an approximately proportionate equal mixture of rutile and anatase. The high temperature phase of titania grows thus even under room temperature processing. After calcination at 400 °C for 4 h, the intensity of the anatase peak grew significantly, indicating a higher anatase ratio. After calcination nitrogen sorption measurements were performed in order to determine the average pore sizes as well as the specific surface areas. The resulting samples were investigated by HRTEM. The samples showed a strong growth anisotropy, i.e. the whiskers revealed a high aspect ratio. The diameter of the whiskers measures approximately 3 – 4 nm and the length up to 50 nm even after calcination. The titania crystals grew as whiskers with a preferential orientation. These needles are aggregated to radial bunches, thus forming nanowhisker arrays.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 219–220, DOI: 10.1007/978-3-540-85226-1_110, © Springer-Verlag Berlin Heidelberg 2008
220
Calcination caused the formation of roundish nanoparticles on top of the whisker tips. These crystalline particles are associated with an amorphous phase and were attributed to the anatase phase. 1. 2. 3.
T. Toyoda, Ikumi Tsuboya, Rev. Sci. Instrum. 74 (1) (2003), p. 782 W. Wunderlich, L. Miao, M. Tanemura, S. Tanemura, P. Jin, K. Kaneko, A. Terai, N. Nabatova-Gabin, R. Belkada, Int. J. Nanoscience 3 (4&5) (2004), p. 439. J. Geserick, N. Hüsing, R. Roßmanith, C.K. Weiß, K. Landfester, Y. Denkwitz, R.J. Behm, U. Hörmann, U. Kaiser MRS Spring Meeting 2007
Figure 1. Left: Survey of nanowhisker arrays in the sample after calcination for 4 h at 400 °C. Right: HRTEM micrograph showing the whiskers with some roundish particles.
d(101) = 0.35nm Figure 2. Left: Roundish particles observed after calcination for 4 h at 400 °C. Right: HRTEM micrograph. Detail of one particle of Fig. 2 left, identified as anatase with 0.35 nm d-spacing of the (101) plane.
221
Quantitative strain determination in nanoparticles using aberration-corrected HREM C.L. Johnson1, E. Snoeck1, M. Ezcurdia1, B. Rodríguez-González2, I. Pastoriza-Santos2, L.M. Liz-Marzán2 and M.J. Hÿtch1 1. CEMES-CNRS, 29, rue Jeanne Marvig, 31055 Toulouse, France 2. Departamento de Quimica Fisica, CSIC, University of Vigo, 36310 Vigo, Spain [email protected] Keywords: strain, nanoparticles, aberration correction, high-resolution electron microscopy
Metallic nanoparticles exhibit exceptional optoelectronic properties that are strongly size and shape dependant and locally variable. Recently, novel synthesis techniques have enabled precise control over the growth of metallic nanoparticles, occasionally resulting in morphologies that cannot be characterized using standard techniques [1]. One example is five-fold-twinned decahedral Au nanoparticles. Owing to the decahedral geometry, these nanoparticles must be strained or contain defects and models have been proposed to predict their strain states. We examined the internal structures of decahedral Au nanoparticles using a combination of aberration-corrected HREM, strain mapping, and finite-element analysis [2,3]. HREM images (Figure 1) were obtained using the SACTEM-Toulouse, a Tecnai F20 ST (FEI) equipped with an imaging aberration corrector (CEOS), rotatable electron biprism and a 2K CCD camera (GATAN). Strain analysis was done using DigitalMicrograph (GATAN) and the GPA Phase 2.0 (HREM Research) software. Microscope distortions were calibrated to obtain highly accurate (< 0.1% strain), highspatial-resolution (< 1 nm) maps of the lattice strain and rotation in the decahedral nanoparticle. Aberration correction provides high-contrast images necessary for accurate high-resolution strain determination. The strain mapping revealed that internal rigid-body rotations (Figure 2a) combined with shear strains (Figure 2b) accommodate the geometric constraints imposed by the decahedral geometry. Our measurements confirm, for the first time, the existence of a disclination. Furthermore, comparison of the results to finite-element analyses revealed that shear strains, which are not predicted by the commonly accepted strain models for decahedral particles, result from elastic anisotropy. The internal structure of these complex nanoparticles will determine their growth and stability as well as affect their surface structures, and, therefore, will be of great importance for engineering their electronic and optical properties. 1. 2. 3. 4.
A. Sánchez-Iglesias et al, Advanced Materials 18 (2006) p. 2529. M.J. Hÿtch et al, Ultramicroscopy 74 (1998), p. 131. C.L. Johnson et al, Nature Materials 7 (2008) p. 120. We thank the EU Integrated Infrastructure Initiative ESTEEM (Ref. 026019 ESTEEM) and the Spanish Ministerio de Educacion y Ciencia (Grants No. MAT2004-02991 and NAN2004-08843-C05-03) for support.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 221–222, DOI: 10.1007/978-3-540-85226-1_111, © Springer-Verlag Berlin Heidelberg 2008
222
Figure 1. Aberration-corrected HREM image of decahedral Au nanoparticle. (a) The image shows the 5-fold rotational symmetry marked by twin boundaries that intersect at the centre of the particle. (b, c) Enlarged views of the core and edge of the particle.
Figure 2. (a) Internal rigid-body rotation of the crystallographic lattice and (b) shearstrain distributions in the decahedral Au nanoparticle. The lattice rotation combined with the shear strains, which result from elastic anisotropy, accommodate the unique geometry of the decahedral particle.
223
Morphological characterization by HRTEM and STEM of Fe3O4 hollow nano-spheres Alfonso Ibarra1, Gerardo F. Goya1, Jordi Arbiol3, Enio Lima Jr.4, Hercílio Rechenberg4, Jose Vargas5, Roberto Zysler5 and M. Ricardo Ibarra1,2 1. Aragon Nanoscience Institute (INA), 2. Materials Science Institute of Aragon (CSICZaragoza University), University of Zaragoza, 50009 Zaragoza, (Spain), 3. TEM-MAT, Serveis Cientificotecnics, UB, 08028 Barcelona, (Spain) 4. LMM, University of São Paulo (Brazil), 5. Centro Atomico Bariloche, 8400, S. C. Bariloche (Argentina) [email protected] Keywords: Fe3O4 nanoparticles, HRTEM, STEM, HAADF, EELS, EFTEM
Morphology, surface and finite size effects in magnetic nanoparticles have been the subject of growing interest in recent years from both experimental and theoretical point of view [1]. The magnetic properties are strongly associated with the morphological and structural homogeneity of the nanoparticles [2]. Interparticle interactions also play an important role in the magnetic behaviour of an ensemble of nanoparticles, which differs from that of non-interacting systems [3]. The aim of this work is the characterization, by means of transmission electron microscopy (TEM), of the morphology and structure of Fe3O4 nanoparticles prepared by chemical route [4] in order to understand their magnetic behaviour. TEM specimens were prepared dispersing the nanoparticles in toluene and dropping this colloidal solution onto a carbon-coated copper grid. TEM analyses were performed in a JEOL 1010 (200 kV). Interesting enough is to point out that a deeper High Resolution TEM (HRTEM) and STEM analysis combined with Energy Filtered TEM (EFTEM) as well as high angular annular dark field (HAADF or Z-contrast) show that magnetite nanoparticles interact creating hollow nano-spheres, and thus affecting the magnetic behaviour of the sample. Figure 1 shows a general view of the sample where the projection reveals a toroidallike shape nanostructures with a weak interaction between them. Electron energy loss spectroscopy (EELS) analyses show that the nanostructures are constituted by Fe3O4, which is corroborated by a chemical analysis where the ~60 % wt. of the final powder corresponds to the Fe3O4 nanoparticles, and ~40 % wt. corresponds to the organic cap of oleic acid that covers the particles and avoid their agglomeration. A more detailed analysis by HRTEM, Figure 2, shows that depending on defocus; new crystallographic planes appear “inside” the projected toroids, indicating that the observed nanostructured may correspond to hollow spheres instead of toroids. In order to confirm this assumption, EFTEM Fe Maps (Figure 3), were obtained showing the homogeneity of the Fe around the whole surface of the sphere. The inferred morphology of hollow spheres is reported here for the first time in magnetic nanoparticles, and it is intimately related to novel magnetic properties displayed by these samples.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 223–224, DOI: 10.1007/978-3-540-85226-1_112, © Springer-Verlag Berlin Heidelberg 2008
224
1. 2. 3. 4. 5.
D. Fiorani., Surface effects in magnetic nanoparticles, Springer, New York (2005). C. B. Murray, C. R. Kagan and M. G. Bawendi, Annu. Rev. Mater. Sci. 30, 545 (2000). J. L. Dormann, E. D'Orazio, F. Lucari, E. Tronc, P. Prené, J. P. Jolivet, D. Fiorani, R. Cherkaoui and M. Nogués, Phys. Rev. B 53, 14291 (1996). J. M. Vargas and R. D. Zysler, Nanotech. 16, 1474 (2005); J. M. Vargas, W. C. Nunes, L. M. Socolovsky, M. Knobel and D. Zanchet, Phys. Rev. B 72, 184428 (2005). This work has been supported by the Spanish Projects Nanoscience Action NAN200409270C3-1/2 and Consolider Ingenio CSD2006-00012. GFG acknowledges support from the Spanish MEC through the Ramon y Cajal program
Figure 1. TEM micrograph of the sample where the projection of nanoparticles seems toroidal structures.
b)
c) 2 nm
a) 5 nm
Figure 2. a) HRTEM micrograph where crystalline planes are observed forming hollow spheres. b) FFT of the area. Welldefined rings show the polycrystalline character of the sample. c) Magnified image of a nanoparticle where the Fe3O4 microstructure is observed.
Figure 3. EFTEM Fe map. The presence of Fe forming the hollow sphere is observed.
225
Direct observation of surface oxidation of Rh nanoparticles on (001) MgO N.Y. Jin-Phillipp, P. Nolte, A. Stierle, P.A. van Aken, and H. Dosch Max Planck Institute for Metal Research, Heisenbergstr.3, D-70569 Stuttgart, Germany [email protected] Keywords: surface oxidation, nanoparticles, HRTEM, EELS, Rhodium
The late transition metals have been studied extensively for decades because of their catalytic applications. Understanding the oxidation behaviour and the structure of the oxides of these metals are essential in order to raise the efficiency of the catalysts [1]. In the present contribution we investigate surface structure of Rhodium (Rh) nanoparticles grown on (001) MgO and oxidized at oxygen (O2) pressure of 2x10-5 mbar by highresolution transmission electron microscopy (HRTEM) in both (110) and (100) crosssections, and by spatially-resolved electron energy-loss spectroscopy (EELS). Surface layer with a structure different from Rh fcc-structure may be clearly seen at the Rh (1 1 1) surface at the top-right side of the particle. As indicated in Figure 1 the measured spacing between the surface layer and the Rh (1 1 1) top layer is 0.28nm, markedly higher than d111,Rh of 0.220nm, measured from the core of the particle. The distance between the image points in the surface layer along <112>Rh is 0.27nm. Similar measurements have been carried out for particles without any surface layer, and it is found that even for the very small Rh particles of a size of ~ 2nm the error is within ±0.005nm. This confirms, that our observation of larger spacing of the surface layer is not due to the deviation of the lattice spacing measurement found in the case of randomly oriented small particles [2]. Spatially-resolved EELS line-scans were performed across {111} surfaces of Rh particles free of epoxy. Figure 2(a) illustrates one of such line scans. Figure 2(b) shows the background subtracted energy-loss near-edge structure (ELNES) of the Rh-M edge of selected spectra. A small extra peak, marked with an arrow, is detected in the spectrum 3 taken at the surface. This small peak lies at the energy position of ~532eV, 11eV distant from Rh-M2 peak, and is therefore the O-K edge. This result suggests that the surface layer observed by HRTEM is surface oxide formed during oxidation. Image simulation using a theoretical model of the surface oxide obtained by density functional theory (DFT) [3] suggests a hexagonal trilayer of O-Rh-O at the Rh (111) surface of the nanoparticles. 1. 2. 3.
H. Over, Y.D. Kim, A.P. Seitsonen, S. Wendt, E. Lundgren, M. Schmid, P. Varga, A. Morgante, and G. Ertl, Science 287 1474 (2000). J.-O. Malm and M.A. O’Keefe, Ultramicroscopy, 68, 13 (1997). J. Gustafson, A. Mikkelsen, M. Borg, E. Lundgren, L. Köhler, G. Kresse, M. Schmidt, P. Varga, J. Yuhara, X. Torrelles, C. Quirós, and J.N. Andersen, Phys. Rev. Lett. 92, 126102 (2004).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 225–226, DOI: 10.1007/978-3-540-85226-1_113, © Springer-Verlag Berlin Heidelberg 2008
226
4.
Financial support from the European Union under Contract No. NMP3-CT-2003-505670 (NANO2) is acknowledged.
Figure 1. High-resolution micrograph of a Rh nanoparticle on the (110) cross-section, showing the surface oxide layer at Rh (1 1 1) surface.
Figure 2. (a) EELS line-scan across the {111} surface of a Rh nanoparticle with a spacing between the spectra of 0.3nm. The scan started at vacuum (spectrum 1) and ended inside the particle (spectrum 7), (b) Selected EELS spectra (3-5) are shown, and an O-K peak is found at the surface (spectrum3).
227
Characterization of catalyst poisoning in biodiesel and conventional diesel fuelled vehicles T. Kanerva1, K. Kallinen2, Toni Kinnunen2, M. Vippola1 and T. Lepistö1 1. Tampere University of Technology, Department of Materials Science, P.O.Box 589, FIN-33101 Tampere, Finland 2. Ecocat Oy, Typpitie 1, FIN-90650 Oulu, Finland tomi kanerva@tut fi Keywords: TEM, catalyst, biodiesel, poisoning
Demand for lower and lower emissions in road transportation has promoted the development of more efficient exhaust emission catalysts. On the same time the fight against the impact of transportation on climate change has opened the way for the use of biofuels, e.g. biodiesel. Deactivation of catalytic surfaces is a serious problem in the design of more efficient automotive exhaust catalysts. Deactivation of catalysts can be classified in three types: chemical (e.g. poisoning), mechanical (e.g. fouling) and thermal (e.g. ageing). In the long run these deactivation processes can cause nearly total loss of catalytic activity in the catalyst material. In biodiesel fuelled vehicles these processes can lead to notably different effects in catalyst efficiency compared to those of conventional diesel vehicles [1]. In this study typical diesel catalyst with noble metals Pt and Pd was vehicle-aged using two different fuels: conventional diesel (EN590) and biodiesel (RME, rapeseed methyl ester). Samples were studied with analytical transmission electron microscope (TEM) and field emission scanning electron microscope (FEG-SEM), both equipped with energy dispersive x-ray spectrometer (EDS). Catalyst poisons from vehicle-ageing were analysed after conventional diesel and biodiesel use. Characterization included EDS-mapping, spot analyses and imaging. According to the results different types and contents of poisons were found in the samples depending on the fuel used. Poisons and their contents are presented in tables 1 and 2. In conventional diesel sample typical poisons were S and K with contents of around 0.5 wt%. In biodiesel samples the highest contents were for poisons S, K and Zn, with much higher proportions. Also overall number of poisons was higher in biodiesel sample. Locations of some EDS-spot analyses for RME and EN590 is presented in figures 1 and 2 respectively. In this vehicle-ageing microstructural effects were minor and no detectable effects were found. In this study the conventional diesel samples were less poisoned and there was not any effect on the performance of this catalyst. The vehicle-ageing using RME caused significant loss of efficiency in the catalyst. Higher contents of poisons and higher number of poisons in vehicle-aged samples using biodiesel rises questions of the quality of biodiesels. There is a lot of research going on to gain more knowledge on the properties and behaviour of biodiesels in automotive engines. Further studies in the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 227–228, DOI: 10.1007/978-3-540-85226-1_114, © Springer-Verlag Berlin Heidelberg 2008
228
effects of biodiesel use on the catalyst components is required to meet the future demands of international energy policies [2]. 1. 2.
J.B. Butt and E.E. Petersen, Activation, Deactivation and Poisoning of Catalysts (Academic Press Inc., 1988). M. Lapuerta, O. Armas and J. Rodriguez-Fernadez, Progress in Energy and Combustion Science 34 (2007), p. 198.
Table 1. Poisons detected in vehicle-aged RME-sample. Contents in wt%. RME
EDS 1 EDS 2 EDS 3 EDS 4 EDS 5 EDS 6 EDS 7 EDS 8
S
0.8
0.2
0.6
0.9
0.1
1.5
1.3
0.2
K
2.4
0.3
4.3
3.7
0.5
2.5
0.9
0.3
0.3
0.1
Ca
0.1
Cr
0.2
0.1
Fe
0.1
0.1
6.2
0.4
0.1
0.3
0.3
Zn
0.5
0.1
0.5
1.1
0.1
0.7
0.9
0.1
Table 2. Poisons detected in vehicle-aged EN590-sample. Contents in wt%. EN590 EDS 1 EDS 2 EDS 3 EDS 4 EDS 5 EDS 6 EDS 7 EDS 8 S
0.5
K Fe Zn
0.2
0.4
0.6
0.4
0.4
0.2
0.1
0.3
0.1
0.1 0.2
Figure 1. Area of RME EDS 1.
0.1
0.1 0.2
0.1
Figure 2. Locations of EN590 EDS 4,5 and 6.
229
TEM Characterisation of Highly Luminescent CdS Nanocrystals Hadas Katz1, Alexey Izgorodin2, Douglas R. MacFarlane2, Joanne Etheridge1,3 1. Dept of Materials Engineering, Monash University, Clayton, Victoria, 3800, Australia 2. ARC Centre of Excellence for Electromaterials Science, Monash University, Clayton, Victoria, 3800, Australia 3. Monash Centre of Electron Microscopy, Monash University, Clayton, Victoria, 3800, Australia hadas katz@eng monash.edu.au Keywords: TEM, Cadmium Sulphide, nanocrystal, electroluminescence.
Luminescent II-VI semiconductor nanocrystals have been the focus of many studies in recent years due to their low energy consumption, wide variety of electroluminescence properties and a large number of combinations of core/shell materials that can be synthesized by the simple and cost efficient reverse micelle method [1]. The size of the nano-crystal determines its surface to volume ratio [2], which affects the band gap and hence the luminescence properties of the crystal. The crystal structure and defect structure, such as point defects and dislocations, also affect band gap energy [3] and hence wavelength of the emitted light as well as the stability of the luminescence materials over time. Characterizing composition, nanocrystals size, crystal structure, defect structure and atomic bonding in the atomic and even subatomic level by electron microscopy will enable us to understand how their size and atomic structure would affect the wavelength of the emitted light and stability of the luminescence materials over time. Those are important factors in the engineering of luminescence materials with desired properties. This work presents an electron microscopy and diffraction study of the crystal structure of highly luminescence CdS nanocrystals produced using the reverse micelles method. Energy-dispersive X-ray spectroscopy (EDX), selected area diffraction (SAD) and atomic resolution imaging using an analytical JEOL 2011 TEM fitted with a LaB6 filament were used to determine the CdS nanocrystal’s composition, crystallographic structure, defect structures and size with a view to understanding how these affect the stability, band gap energy and luminescence properties. Nanoparticles were observed both aggregated in clusters and distributed across the carbon film. The size of the nanoparticles is typically between 3-13nm and was determined by counting of atomic planes in atomic resolution images. Selected area diffraction (SAD) patterns taken from filtered solution indicate the presence of hexagonal CdS and cubic CdS only. However, in unfiltered solutions cubic
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 229–230, DOI: 10.1007/978-3-540-85226-1_115, © Springer-Verlag Berlin Heidelberg 2008
230
CdO and cubic Na2S nanocrystals were also observed and are assumed to be byproducts. Careful measurement of a SAD pattern of numerous particles distributed across the carbon film shows a 4% difference in the nominal cubic 220 and -220 spacing, suggesting the cubic CdS structure is distorted. This could have an affect on band gap and electroluminescence properties. Using high resolution images and their Fourier transforms, it was conformed that both cubic and hexagonal CdS nanocrytals and a cubic CdO by–product are produced using the reverse micelle process (e.g. figure 1). In addition, a high resolution image of a small cluster containing 3 cubic CdS nanocrystals shows that these particles share a common atomic plane and might had inter-grown during growth process. 1. 2. 3.
D. R. Vij, Handbook of Electroluminescent Materials, Institute of Physics Publishing, (2004). S. J. Rosenthal, J. McBride, S. J. Pennycook, L.C. Feldman, Surface Science Reports, 62 (2007) 111-157. Ronghui Xu, Yongxian Wang, Guangqiang Jia, Wanbang Xu, Sheng Liang, Duanzhi Yin,. Journal of Crystal Growth, 299 (2007) p. 28-33.
Figure 1. (a) HRTEM Image of A small cluster of 4 CdS nanocrystals supported on a carbon film. (b) Fourier transform taken of the image. 3 nanoparticles have cubic structure and are oriented down the <103> and <112> zone axis and share the {31-1} atomic plane (fig. b1). The fourth nanoparticle has hexagonal CdS structure (fig. b2). (c) Inverse of the Fourier transform with diffuse background masked to enhance atomic contrast. The orientations of the 3 cubic CdS nanocryatls sharing the {31-1} atomic plane (fig c1) and of the hexagonal CdS nanocrystal atomic plane (fig. c2) are marked. The cluster diameter is ~7 nm.
231
Structure and composition of dilute Co-doped BaTiO3 nanoparticles O.I. Lebedev, R. Erni and G. Van Tendeloo EMAT, University of Antwerp, Groenenborgerlaan 171, B2020 Antwerpen, Belgium [email protected] Keywords: nanoparticles, edge dislocation, vacancies, EFTEM, HRTEM
Dilute ferromagnetism in semiconductors with Curie temperatures (Tc) above 300 K are materials of high technological interest due to their potential use in spin based electronic devices operable at room temperature. Additionally, the current technological trends towards device miniaturization are driving the development of materials research strongly in the direction of functional nanomaterials. Therefore, fabrication of well characterized nano dilute magnetic semiconductor systems is becoming increasingly important. Nanoparticles of 5% Co-doped BaTiO3 (Co-BTO) with nominal composition BaTi1¡xCoxO3 were synthesized following an established solvothermal drying route with additional cobalt(II) nitrate hexahydrate as Co precursor in stoichiometric quantities. Detailed TEM and ED studies confirm that the samples are indeed single phase Codoped BaTiO3, devoid of other impurity phases or Co metal clusters. HRTEM investigation indicates the presence of Ba vacancies in varying concentrations. Figure 1 shows a HRTEM image from a single Co-BTO nanoparticle along the [111]C zone axis. There is a clear reduction of contrast of the lattice fringes within 1-2 nm size areas. Such local variation in HRTEM contrast can be attributed to clusters of Ba vacancies. Moreover, exceeding a certain vacancy concentration leads to internal stress that can be reduced by the formation of edge dislocations (Fig.2a). The existence of dislocations is particularly surprising in case of nanoparticles where the energy stability of a dislocation is not a priori warranted. The closure failure of the Burgers circuit in the HRTEM image (Fig.2b) determines the Burgers vectors as b1 and b2 =a√2 [110]C (a being the lattice parameter of cubic BaTiO3). In order to clarify the origin of these contrast variations, EFTEM and Z- contrast imaging have been employed. The EFTEM Ti and Co map (Fig 2d,e) clearly confirms a quite narrow Ti-Co distribution inside the nanoparticles while the Z-contrast imaging (Fig.2c) indicates that the bright spots correspond to pore-like structures in the nanoparticles, and are not related to any chemical inhomogeneity or metal clustering effects. The elemental maps and the plasmon-loss image reveal that the regions with brighter contrast in the HRTEM image do not correlate with increased concentrations of Ti or Co. This leads to the conclusion that physical voids within the particles have to be present. Electron Microscopy results indicate that we have formed Co-doped cubic BTO nanocrystals in which the presence of vacancies and relative defect concentrations regulate the occurrence/absence of ferromagnetism.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 231–232, DOI: 10.1007/978-3-540-85226-1_116, © Springer-Verlag Berlin Heidelberg 2008
232
Figure 1. [111] HRTEM image of Co-doped BaTiO3 nanoparticle and corresponding FT pattern. Filtered HRTEM image from selected region marked by white frame notice variation of the contrast ( marked by white arrow)
Figure 2. (a) - [111] HRTEM image of a highly defected Co-doped BaTiO3 nanoparticle and corresponding FT pattern; (b)-filtered HRTEM image showing presence of core dislocations. The associated Burgers circuits are indicated. (c) - Z contrast image of an agglomerate of nanoparticles exhibiting inhomogenities and EFTEM images of selected nanoparticles at Co-M edge(65 eV energy loss) (d) and TiM edge (45 eV energy loss) (e)
233
CoxFe3-xO4 catalytic materials for gaz sensors L. Ajroudi1,2, A. Essoumhi1, S. Villain1, V. Madigou1, N. Mliki2, and Ch. Leroux1 1. IM2NP (UMR-CNRS 6242), South University Toulon-Var (USTV), Bat.R, B.P.20132, 83957 La Garde Cedex, France 2. LMOP, Physics Department, University Tunis El-Manar, 2092 Tunis, Tunisia [email protected] Keywords: nanoparticles, ferrites, catalysis
Nanomaterials based on spinel ferrites have already numerous applications, mainly based on their magnetic properties. Recently, catalytic properties of nickel, copper and cobalt ferrites in the conversion of CO and CH4 were evidenced, opening a new field of applications for these materials [1]. Magnetic properties of nanoparticles, as well as catalytic properties, will depend on their size, but also on their shape and size distribution. These parameters are linked to the elaboration method. The properties of transition metal spinel oxides depend also on the nature of the transition metal and on his site occupation in the structure. The location of the cations in the spinel structure is related to their octahedral or tetrahedral sites preference, but also to the synthesis method. For magnetite Fe3O4, which adopts the inverse spinel structure, the tetrahedral sites are fully occupied by Fe3+ ions, whereas octahedral sites are occupied by Fe3+ and Fe2+. For Co3O4, the octahedral and tetrahedral sites are respectively occupied by Co3+and Co2+ (normal spinel structure). Intermediate situations occur for CoxFe3-xO4 ,. Thus, three different compositions were prepared CoFe2O4, Co0 6 Fe2 4O4, Co1 4 Fe1 6O4. In order to synthesize chemical homogeneous powders, we used a co-precipitation method, and a non aqueous elaboration technique developed by Pinna [2]. For the coprecipitation method, the starting iron and cobalt salts were FeCl3.6H2O, FeSO4.7H2O and CoSO4.7H2O. Two different co-precipitations were realised. The proportions and nature of the salts changed, but the rest of the procedure was the same. The salts were dissolved in distilled water, and the solution was then mixed to a solution of NaOH, heated at 70°C. Since Fe3O4 was obtained by co-precipitation of FeCl3.6H2O and FeSO4.7H2O, a co-precipitation was realised with FeCl3.6H2O, FeSO4.7H2O, and CoSO4.7H2O, (sample A FC 17). Another attempt with FeCl3.6H2O and CoSO4.7H2O, was also done (sample B FC16). The precipitates were annealed at different temperatures (250°C,300° and 500°C). For the second method, iron acetylacetonate and cobalt 2,4-pentanedionate were mixed in various proportion in benzyl alcohol. The mixture was stirred and put into a steel autoclave. After two days in a furnace, one obtains a dark suspension, which was ultrasonicated and centrifuged. The precipitates were thoroughly washed and subsequently dried in air. This procedure was applied to the elaboration of CoFe2O4 (sample C), Co0 6 Fe2 4O4,(sample D) and Co1 4 Fe1 6O4 (sample E). Whatever the elaboration method, CoxFe3-xO4 nanoparticles were obtained. The spinel nanoparticles, obtained by co-precipitation method, have irregular shapes (Figure 1a) and mean sizes ranging from 8 nm (sample B, 300° C) to 12 nm (sample A, 500 °C).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 233–234, DOI: 10.1007/978-3-540-85226-1_117, © Springer-Verlag Berlin Heidelberg 2008
234
Sample B is chemically homogeneous, but sample A contains Co3O4 in form of platelets and needles (Figure 1b). TEM studies of samples annealed at lower temperatures showed that the platelets result from the decomposition of cobalt hydroxide, as needles come from the initial cobalt sulphate. Spinel nanoparticles obtained by the non aqueous method are very regular in shape and well dispersed (Figure 2a). They are also chemically homogeneous and very homogeneous in size (Figure 2b). The chemical composition was tested by nanoprobe analysis. 1. 2.
D. Fino, S. Solaro, N.Russo, G. Saracco, V. Specchia, Topics in Catalysis 42, (2007), p.454 N. Pinna, S. Grancharov, P. Beato,| P. Bonville, M. Antonietti and M. Niederberger, Chem. Mater. 17 (2005), p. 3044.
Figure 1. a) HREM of one CoFe2O4 particle, with a [110] zone axis. b) Sample A, annealed at 500°C. The powder consists in a mixture of CoFe2O4 nanoparticles, and Co3O4, in form of platelet and needles.
Figure 2. a) CoFe2O4 nanoparticles (sample C). b) Histogram of the size distribution.
235
(S)TEM investigation on the role of alumina dopants to prevent redox activity decay at high temperature in CePrOx /doped-Al2O3 catalysts M. López-Haro, K. Aboussaid, J.M. Pintado, J.J. Calvino, S. Trasobares Departamento de Ciencias de los Materiales, Ingeniería Metalúrgica y Química Inorgánica. Universidad de Cádiz, 11510-Puerto Real (Cádiz). Spain [email protected] Keywords: CePrOx Catalysts, STEM, doped-alumina
CePrOx mixed oxides, which present extraordinary redox properties, have a wide range of potential applications in environmental catalysis [1]. A good dispersion of these oxides over a high surface area material, like alumina, increases their specific surface and, hence, their oxygen handling capabilities. Moreover if the alumina support is modified with a doping agent, their textural stability can be improved and their deactivation by solid-state reaction with the support inhibited [2]. In this work, Transmission Electron Microscopy Imaging Techniques (HREM and HAADF) have been combined with spectroscopic techniques, (EELS and X-EDS), to investigate the influence of the dopant nature (SiO2, La2O3) on the chemical and structural properties of CePrOx particles supported on modified aluminas. A mechanism to explain the differences observed [3] in the resistance against high temperature deactivation of a Ce0 8Pr0 2O2-x supported on Si-doped alumina (Ce0 8Pr0 2O2-x/Al2O3- 3.5% SiO2) and a La-doped alumina (Ce0 8Pr0 2O2-y/Al2O3 -4% La2O3) system is proposed. To reveal the effects of high temperature aging, samples of the two catalysts were studied after treatments under reducing conditions at low, 350ºC, and high temperature, 900ºC. HREM indicates the presence in both materials of a fluorite-like structure on the samples treated at 350ºC. Neatly different results are observed at the highest temperature. Thus, two different crystalline phases have been detected in the Si-doped material: a lanthanide hidroxycarbonate (Bastnesite-type) (figure 1.A) and a fluorite-like structure. In the case of La-doped sample, only a perovskite phase, LnAlO3 (Ln=Ce, Pr) (figure 1.B) is observed. The formation of the redox-inactive perovskite phase would explain the greater deactivation behaviour observed in the La-doped sample. To investigate further the role of the dopant in these solid state chemistry differences, the samples were characterised by STEM-XEDS and STEM EELS. These techniques provide a more accurate, high spatial resolution, description of the elements distribution. In the Si-doped samples (both at 350ºC and 900ºC) EELS studies indicated the simultaneous presence of small (a few nanometers) PrOx crystallites and, much larger (100-200 nm), Ce-rich, CePrOx crystals over the support. In contrast, in the La dopedsample, Pr is homogeneously distributed all over the catalyst, not only in the form of Ce-rich CePrOx mixed oxide particles (at low temperature) or as LnAlO3 (at high temperature) but also into/over the alumina particles (figure 2).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 235–236, DOI: 10.1007/978-3-540-85226-1_118, © Springer-Verlag Berlin Heidelberg 2008
236
These results suggest that the addition of SiO2 as dopant prevents the formation of the redox-inactive LnAlO3 perovskite phase by blocking the diffusion of the lanthanide ions into the alumina crystallites, which allows maintaining the lanthanide ions within crystalline phases which still present a high enough Ln4+/Ln3+ exchange capability.
Figure 1.- Experimental HREM images acquired on (a) the Si-doped material and (b) the La-doped material reduced at 900ºC. Ce M5,4 La M5,4
Pr M5,4
1050
0
950
50
Distance (nm)
100
850
Energy Loss (eV)
Figure 2.- EELS 3D representation of a collection of 50 spectra acquired on the Ladoped material after treatment at 900ºC. Similar results were observed at 350ºC. 1. 2. 3. 4.
M. Shelef, G.W. Graham, R.W. McCabe, Catalysis by Ceria and Related Materials A. Trovarelli,Imperial College Press, London 343-374 (2002). H. Schaper, E. B. M. Doesburg, L.L. van Reijen, Appl. Catal. 7, 211 (1983). K. Aboussaid, S. Bernal, G. Blanco, G.A. Cifredo, A. Galtayries, J.M. Pintado Mohamed Soussi el Begrani. Surface and Interface Analysis, 40, 3-4 ,250-253 (2008) We acknoledge the financial support from Ministry of Education and Science of Spain (Proyto MAT2005-00333) Junta de Andalucía (Grupos FQM-110 y FQM-334), and Programa Ramón y Cajal 2003. The electron microscopy work was carried out at the Electron Microscopy Division of Central Services of Science and Technology at the University of Cádiz.
237
Sulfated Zirconia Catalysts: Structure and Performance Relationship, a TEM Study C. Meyer1, D. Su1, N. Hensel1, F.C. Jentoft1 and R. Schlögl1 1. Department of Inorganic Chemistry, Fritz-Haber Institute of the Max Planck Society, Faradayweg 4-6, 14195 Berlin, Germany [email protected] Keywords: Sulfated zirconia, structure, heterogeneous catalysis, HR-TEM
Sulfated Zirconia (SZ) is an important and suitable catalyst for heterogeneous nalkane isomerization that experiences braod industrial application. Zirconia in tetragonal phase that is stabilized at low temperature in the form of nanosized particles [1] proved a high activity and selectivity for this reaction [eg. 2]. A key issue in elucidating parameters relevant for catalytic performance is the observation of processes occurring during the calcination process, in which the precursor material is transformed to the active catalyst [3]. During calcination exothermic crystallization of the amorphous zirconia precursor produces a specific overshoot in the temperature known as the glow phenomenon. Once this event has occurred, the material exhibits significant activity as opposed to the inactive precursor. This study is focused on the correlation of structural characteristics and activity or selectivity of SZ nano powder catalyst. A series of quenching experiments at different stages of the calcination process has been conducted. Sulfated hydrous zirconia (MEL Chemicals XZ0 682/01) was used as starting material. Calcination was performed in flowing air at 823 K in batches of 20 g. Temperature was held for 3 h, applying a temperature ramp for heating and cooling of 15 K / min. Quenching in liquid nitrogen was done before, during and after the glow phenomenon as well as at completion of the temperature program. Isomerisation of nbutane (1 % n-butane in He at atmospheric pressure) at 373 K was used as a test reaction. Activity and selectivity of the catalyst samples were monitored as a function of time by on-line gas chromatography. Further characterization included XRD, UV-VIS and BET measurements. Systematic TEM investigations reveal sample properties with a high degree of spatial resolution. Electron diffraction and Fourier transformation are used for phase characterization, EDX and EELS for chemical analysis and HR TEM for morphology and grain size measurements. Further, detailed structures of single grains are investigated. Figure 1 exhibits features of interest using a tetragonal grain of zirconia with a maximum diameter of 30 nm as an example. Line of sight is parallel to [100], (011) and (002) are projected. Surface steps (1), bending of projected lattice traces (2) and intra grain porosity (3) are observable. This sample is taken after the glow phenomenon and shows high activity. Figure 2 shows for comparison a sample with little catalytic activity. Lattice spacings
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 237–238, DOI: 10.1007/978-3-540-85226-1_119, © Springer-Verlag Berlin Heidelberg 2008
238
prove the tetragonal nature of the zirconia. A difference lies for example in the smoothness of the surface termination denoting energetic differences.
Figure 1. HR TEM micrograph of SZ catalyst. Projection of (011) and (002), line of sight is [100]. The arrows indicate exemplarily structural features, for details see text.
Figure 2. HR TEM micrograph of SZ catalyst. (011) planes of tetragonal zirconia are projected. The arrows indicate porosity (1) and a smooth surface termination (2). 1. 2. 3.
R.C. Garvie, J. of Phys. Chem., 82 (1965), p. 218 – 224. M. Benaissa, J.G. Santiesban, G. Dias, C.D. Chang, M. Jose-Yacaman, J. of Catalysis, 161 (1996), p. 694 - 703. A.H.P. Hahn, R.E. Jentoft, T. Ressler, G. Weinberg, R. Schlögel, F.C. Jentoft, J. of Catalysis, 236 (2005), p. 324 - 334.
239
A novel procedure for an accurate estimation of the lattice parameter of supported metal nanoparticles from the analysis of plan view HREM images C. Mira, J.A. Perez-Omil, J.J. Calvino and S. Bernal Dep. Ciencia de los Materiales e Ingeniería Metalúrgica y Química Inorgánica. Universidad de Cádiz. c/ Rep. Saharaui s/n. 11510 Puerto Real (Cádiz) - SPAIN cesar [email protected] Keywords: HREM, plan view, nanoparticle lattice parameter
The lattice parameter of metal nanoparticles supported on a carrier material, as are those present in a large variety of catalysts, can suffer small modifications from the value expected for the bulk materials. Thus, dilatation or contraction of the lattice constant of supported metal has been related to effects like incorporation of support elements into the particles in the form of alloys; incorporation of small atoms of other elements, like H, O, or C, into the metal lattice; pseudomorphic growth; surface stress or encapsulation of the metal under a large compressive stress by the substrate. The observed modifications of the lattice parameter are frequently smaller than 5%. A precise quantification of this effect could help to understand their precise origin. The measure of lattice parameters by X-ray diffraction is quite extended. In spite of its accuracy this technique provides only an average value of all the particles under analysis. Likewise, the analysis becomes very unreliable with diffraction patterns with a low signal to noise ratio as are those obtained in systems with very small particles. In the case of HREM images, errors higher than 5% can be expected in direct measurement of lattice spacings [1]. In fact, the accuracy with this measurement technique depends on several experimental factors [2]. SAED patterns allow estimations with high relative errors (2-3%). An statistical approach, considering a large number of particles, improves the accuracy of HREM or SAED measurements [3], but in this case we are not characterising a single particle but an ensemble of them. We have developed a procedure to increase the accuracy in the determination of the lattice spacings of supported metal particles based on the detailed analysis of Moiré type fringes observed in plan view HREM images. These Moiré fringes correspond to linear combinations between the characteristic metal and support reflections. With particles of only a few nanometers a large number of Moiré spots can be detected in the corresponding image diffractograms. Using the lattice fringes of the bulk support as a reference, the measurement of each Moiré reflection in reciprocal space allows an estimation of metal lattice spacings. The error obtained in these individual determinations is lower than that expected for the direct measurement of the metal spacing, the exact value of the error depending on the specific Moiré reflection selected. Nevertheless, a much better estimation can be obtained if all the information present in the diffractogram is used simultaneously.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 239–240, DOI: 10.1007/978-3-540-85226-1_120, © Springer-Verlag Berlin Heidelberg 2008
240
If we record an intensity profile of the image diffractogram we can try to fit it to a theoretical curve in which the metal structure is the parameter to be refined. We have developed a software to apply this approach. This program allows us fitting simultaneously all the visible peaks in the intensity profile, which includes not only the metal and support peaks but also a set of Moiré reflections. The positions of the different peaks in the theoretical curve are very sensitive to subtle modifications of the metal lattice spacings. Thus, the correlation coefficient between the theoretical and experimental curves shows a maximum for a precise metal spacing value, usually corresponding to situations of slight lattice contractions or expansions. In the figure below a planar view of a CeO2-supported Pd particle (a) and its diffractogram (b) are shown. Different Moiré reflections can be identified, which result from the combination of (111) CeO2 and (111) Pd reflections. The experimental intensity profile and its theoretical fitting are also shown. Two possible metal lattice modifications have been considered (c). A 0.6% contraction shows a better correlation (r) than that characteristic of a 0.4% expansion. By applying this procedure to the analysis of HREM images simulated for a set of models which consider exact metal lattice expansions/contractions we have estimated the precision of the method to be of the order of 0.2%. This new procedure has been applied to Pd/CeO2 images to detect, in single particles, variations in the metal lattice parameters lower than 1% with high reliability. 1. 2. 3. 4.
J.-O. Malm, M.A. O´Keefe; Ultramicroscopy 68 (1997) 13-23. W.J. DE Ruijter, R. Sharma, M.R. McCartney, D.J. Smith; Ultramicroscopy 57 (1995) 409422 S.-C.Y. Tsen, P.A. Crozier, J. Liu; Ultramicroscopy 98 (2003) 63-72 MEC/FEDER (MAT2005-00333) and JA (FQM-110, FQM-334) are acknowledged
a
b CeO2 Pd
Figure 1. (a) HREM image of a Pd/CeO2 catalyst ; (b) image diffractogram; (c) fitting of the experimental intensity profile to -0.6% and 0.4% variations in the lattice parameter. 300
300
-0,6%
r = 99,2%
250
r = 98,3%
250
+0,4%
Calc exptal.
200
intensity
intensity
200 150 100
100 50
50
0
0
c
150
0
20
40 pixel
60
80
0
20
40 pixel
60
80
241
Microstructure of Pt particles and aggregates deposited on different carbon materials for fuel cells application D. Mirabile Gattia1, E. Piscopiello1*, M. Vittori Antisari1, S. Bellitto2, S. Licoccia2, E. Traversa2, L. Giorgi1, R. Marazzi1, A. Montone1 1. FIM Department, ENEA – C.R. Casaccia, Via Anguillarese 306, 00123 Rome, Italy *C.R.Brindisi, Via Appia Km 702, 72100 Brindisi, Italy 2. Department of Chemical Science and Technology, University of Roma “Tor Vergata”, Via della Ricerca Scientifica, 00133 Rome, Italy daniele [email protected] Keywords: carbon nanostructures, fuel cell, catalyst
PEM (polymer electrolyte membrane fuel cells) and DMFC (direct methanol fuel cells) have demonstrated to be suitable devices in order to realize a widespread diffusion of electrical-H2 fed vehicles in the near future [1]. In recent years several research efforts were on the study of Pt clusters deposited on different kinds of nanostructured carbon, besides the classical carbon black, with the purpose of reducing the Pt loading by the optimization of the catalyst performances during electrochemical reactions at the cell electrodes. In this work Pt clusters have been deposited by an impregnation process on three carbon supports: Multi-Wall carbon Nanotubes (MWNT), Single-Wall carbon Nanohorns (SWNH) and Vulcan XC-72. MWNT and SWNH have been home synthesized by a DC [2] and an AC arc discharge process [3] respectively. The Pt particles, deposited on the three carbon supports, have been characterized by Scanning and Transmission Electron Microscopy, X-ray diffraction and cyclic voltammetry measurements. Electron microscopy investigations, revealed the presence of nanostructured aggregates with different diameters: 50-100 nm and 20-50 nm in Pt/SWNH and Pt/MWNT samples respectively, while in the case of Pt/Vulcan single nanoparticles were deposited. In this last sample the process resulted in a strongly inhomogeneous microstructure with several sample regions free from deposited particles. Electrochemical characterization showed that the Pt nanostructures deposited on MWNT were particularly efficient in the methanol oxidation reaction, even if the Pt active surface area on the Vulcan substrate is larger. This shows that particle aggregates can be more efficient respect to single particles, probably owing to the particular particle shape and to the presence of grain boundaries. The comparison between the two nanostructured substrates evidences furthermore a role for the small size of aggregates. The details of the microstructure, as evidenced by the high resolution TEM analyses, are reported in the insets (figure 1). The agglomerates deposited on the nanotubes appear to be constituted by single crystal region larger than the single leafs so that the structure appears quite complex and requires further analyses for a complete description.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 241–242, DOI: 10.1007/978-3-540-85226-1_121, © Springer-Verlag Berlin Heidelberg 2008
242
a)
b)
c)
d)
Figure 1. Low magnification (a) and high magnification (b) TEM images of Pt particles deposited on Vulcan XC-72. In the inset a high resolution image is reported. In (c) and (d) Pt aggregates deposited on MWNT are shown with a high resolution detail in the inset. 1. 2. 3.
S. Gottersfield and T. Zawodzinski, Adv. Electrochem. Sci. Eng. 5 (1997), p. 195. D. Mirabile Gattia, M. Vittori Antisari, R. Marazzi, L. Pilloni, V. Contini and A. Montone, Materials Science Forum 518 (2006), p. 23. D. Mirabile Gattia, M. Vittori Antisari and R. Marazzi, Nanotechnology 18 (2007), p. 255604.
243
Low-loss-energy EFTEM imaging of triangular silver nanoparticles J. Nelayah1, L. Gu1, W. Sigle1, C.T. Koch1, L. Pastoriza-Santos2, L.M. Liz-Marzan2, and P.A. van Aken1 1. Max Planck Institute for Metals Research, Stuttgart Center for Electron microscopy, Heisenbergstr. 3, D-70569 Stuttgart, Germany 2. Departemento de Quimica Fisica, Universidade de Vigo, 36310, Vigo, Spain nelayah@mf mpg.de Keywords: EFTEM, EELS, metallic nanoparticles, surface plasmon mapping
Understanding how light interacts with matter at the nanometer scale is a fundamental issue in optoelectronics and nanophotonics. It is known that the optical properties of nanoparticles are entirely dependent on collective excitations of their valence electrons, known as "surface plasmon resonances" (SPR´s), under electromagnetic illumination. Measuring these properties locally at the level of the individual nano-object constitutes a challenging issue for linking of the global response of the nanoparticles and the underlying structure and morphology. The high-energy electron beam in a transmission electron microscope (TEM) is an excellent tool for this application. In particular, it has been recently shown that low-loss electron energy-loss spectroscopy (EELS) in the context of a scanning transmission electron microscope (STEM) enables the optical properties of metallic nanoparticles in the ultraviolet–near-infrared (UV–NIR) domain to be probed with nanometer resolution via the mapping of SPR´s [1]. With the advent of recent instrumental improvements such as electron monochromators and in-column energy filters, it is expected that the understanding of these optical properties can be further improved through the gain in both energy and spatial resolution. In this contribution, we present energy-filtered transmission electron microscope (EFTEM) studies of the optical properties in the UVNIR regime of individual triangular silver nanoparticles.. Triangular silver nanoprisms have been synthesized as described in [2]. The prisms have edge lengths in the range between 100 and 300 nm and are typically between 5 and 10 nm thick. The instrument used for this investigation was the new 200 kV SESAM FEG-TEM (Zeiss) fitted with an electrostatic monochromator and a high-dispersion and high-transmissivity in-column MANDOLINE filter [3]. The energy resolution was set to 0.25 eV for these experiments. The EFTEM series were acquired on a 2k × 2k CCD camera (8 × 8 binning) using a 0.2 eV energy selecting slit. Energy-filtered images were recorded from 0.5 eV to 4 eV (17 images) with an acquisition time of 20 s/image. Figure 1 shows a series of EFTEM images of a triangular nanoparticle with 210 nm edge length recorded at energy losses of (a) 0 eV, (b) 1.0 eV, (c) 1.6 eV, and (d) 2.2 eV, respectively. The two-dimensional images in Figures 1(b)-(d) represent the intensity distributions of the first three main SPR´s of the silver nanoprism as already observed with STEM-EELS in [1]. But, compared to the latter data, our EFTEM images display
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 243–244, DOI: 10.1007/978-3-540-85226-1_122, © Springer-Verlag Berlin Heidelberg 2008
244
increased spatial sampling and are obtained with shorter acquisition time and without post-acquisition data processing. These results clearly demonstrate that low-energy-loss EFTEM imaging in the SESAM microscope provides a fast and precise analytical tool for investigating the optical properties of single metallic nanoparticles in the visible range. This tool enables both unprecedented spatial and energy resolution which will provide new information about the optical properties of nanomaterials. 1. 2. 3. 4.
J. Nelayah, M. Kociak, O. Stephan, F.J.G. de Abajo, M. Tencé, L. Henrard, D. Taverna, I. Pastoriza-Santos, L.M. Liz-Marzan, and C. Colliex., Nature Physics 3 (2007) 348. V. Bastys, I. Pastoriza-Santos, B. Rodriguez-Gonzalez, R. Vaisnoras and L.M. Liz-Marzan, Adv. Funct. Mater. 16 (2006) 766. C.T. Koch, W. Sigle, R. Höschen, M. Rühle, E. Essers, G. Benner, and M. Matijevic, Micoscopy and. Microanalysis 12 (2006) 506. We acknowledge financial support from the European Union under the Framework 6 program under a contract for an Integrated Infrastructure Initiative. Reference 026019 ESTEEM
(a)
(b)
(c)
(d)
Figure 1. EFTEM images of a triangular silver nanoparticle with 210 nm edge length imaged at energy losses of (a) 0 eV, (b) 1.0 eV, (c) 1.6 eV and (d) 2.2 eV. Images were taken with a slit width of 0.2 eV centred on the specific energy loss. Scale bar and colour level are common for all images. The bright pixels indicate maximum intensity.
245
Microstructure of cobalt nanocluster arrays fabricated by solid-state dewetting Yong-Jun Oh1, Junghwan Kim1, Sukhun Hwang1, Caroline A. Ross2, Carl V. Thompson2 1. Advanced Materials Science and Engineering Div., Hanbat University, Korea 2. Department of Materials Science and Engineering, Massachusetts Institute of Technology, Cambridge, Massachusetts 02139 [email protected] kr Keywords: nanoclusters, dewetting, cobalt phases
Cobalt nanocluster arrays have recently attracted considerable attention due to their applications as patterned magnetic recording media as well as catalyst arrays for growing carbon nanotubes [1,2]. The processes to fabricate nanocluster arrays are mostly based on direct lithography of thin films using coatings of photo resist and their selective removal. Since the resultant clusters formed by this technique retain the microstructure of the original thin films, we need to control the microstructure of thin films before lithography to obtain clusters with specific crystal property. Recently, one of the authors developed a self-assembling technique to fabricate gold nanoparticle arrays by dewetting a thin metal film on topographic templates at elevated temperatures [3]. The technique was also characterized by crystal reorientation during agglomeration of the thin film by dewetting. In this study, we investigate the changes in phase, crystallography, and microstructure of cobalt before and after dewetting by thermal annealing. The topographic templates consisted of 200-nm-period square arrays of inverted pyramidal pits on (100) silicon wafers. Interference lithography using a laser beam was used to create patterns on the wafers. The templates were oxidized to prevent the reaction between the substrate silicon and the cobalt thin film. The cobalt films were deposited on the templates using ion-beam sputtering and were annealed in forming gas to induce dewetting. The ordered cobalt clusters at a high temperature were mostly in the fcc phase (Figure 1), while the films annealed at a low temperature showed a mixture of hcp and fcc cobalt phases (Figure 2). The dewetted clusters were almost single crystal when twin boundaries were disregarded. The orientation of more than a quarter of the observed particles was such that the (111) plane of the Co particles was parallel to a pair of the inverted pyramidal faces of the silicon template. The dewetting process is believed to be a promising technique to fabricate single-crystal nanocluster arrays for high-density magnetic recording media and carbon nanotube growth. 1.
J.I. Martin, J. Nogues, K. Liu, J.L. Vicent, I.K. Schuller, Journal of Magnetism and Magnetic Materials 256 (2003), p.449.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 245–246, DOI: 10.1007/978-3-540-85226-1_123, © Springer-Verlag Berlin Heidelberg 2008
246 2.
3. 4.
C.A. Ross, M. Hwang, M. Shima, J.Y. Cheng, M. Farhoud, T.A. Savas, Henry I. Smith, W. Schwarzacher, F.M. Ross, M. Redjdal, F.B. Humphrey, Physical Review B, 65 (2002), p.144417. A.L. Giermann, C.V. Thompson, Applied Physics Letters 86 (2005), p.121903. We thank H.I. Smith and K. Berggren at MIT for interference lithography. (a)
(b)
Zfcc-Co=[110]
100 nm
100
Figure 1. (a) Scanning and (b) transmission electron microscope (SEM and TEM) images showing the dewetted clusters. The SAD pattern on the top right was taken from the particles in pits.
fcc[100]
fcc[110]
hcp[1213]
5 nm
Figure 2. High-resolution TEM image of the as-sputtered cobalt film. The arrows indicate the grains of fcc-Co and hcp-Co phases showing the atomic images along zone axis with low indices.
247
Size Effect in Gold Nanoparticles Investigated by Electron Holography and STEM L. Ortolani1,2, V. Morandi2 and M. Ferroni3 1. University of Bologna, Dept. of Physics, v.le B. Pichat, 6/2, 40127 Bologna, Italy 2. CNR-IMM Bologna, v. Gobetti, 101, 40129 Bologna, Italy 3. INFM-CNR SENSOR and Dept. of Chemistry and Physics, Brescia University, v. Valotti, 9, 25133 Brescia, Italy [email protected] Keywords: Gold Nanoparticles, Electron Holography, HAADF-STEM
Gold clusters are extremely interesting nanosystems with a high catalytic activity, exploited for sensing applications and to promote the growth of nanostructures [1,2]. All these potential applications motivated numerous structural studies on Au nano-clusters. The mean electrostatic potential (MIP) is a fundamental quantity and its value is crucial for accurate evaluation and simulation of experimental data from TEM imaging and electron diffraction. Recently, a dependence of the MIP on particle size has been reported, measured by electron holography (EH): the increase of the MIP over the bulk value for particle sizes lower than 5 nm has been shown, suggesting a correlation with the catalytic behaviour of gold [3,4]. Despite these very promising results, a similar effect was observed in amorphous carbon films as the result of a thickness independent phase shift [5]. EH is capable of providing a quantitative determination of this surface phase shift since it depends on the projected sample thickness. Unfortunately, gold particles are reported to change their contact angle with the substrate reducing their dimension, as a result of a size-dependent change in the particle-support interaction [3]. To overcome these limitations, and to determine unambiguously information on surface phase effects in gold clusters, a combination of High Angle Annular Dark Field STEM (HAADF-STEM) and electron holography has been used, exploiting the local sample thickness dependence of the HAADF-STEM signal. HAADF intensity depends also on the imaging conditions, on the atomic number and of the density of the observed material. By keeping fixed all these parameters, it is possible to directly correlate image intensity to sample thickness variations. From the holographic reconstructed phase map of gold clusters over an amorphous carbon film, like the one shown in Fig. 1a), it is possible to fit the induced phase shift and the projected radius of the particle, as reported in the linescan of Fig. 1b). From a HAADF-STEM image of the same clusters it is possible to fit the projected radius and the HAADF intensity, as shown in Fig. 2a). By keeping constant all the imaging parameters, intensity variation in the image only depends on changes in the particles shape. The fit of the data of Fig. 2b) shows that the smaller particles are thinner than the larger ones, as shown in the model of Fig. 3a). From these results it is possible to correct the electron holography phase shift measurements, obtaining the plot of Fig. 3b). Numerical fitting of the data reveals, for gold clusters dispersed over a carbon film, a thickness independent phase shift of 0.45
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 247–248, DOI: 10.1007/978-3-540-85226-1_124, © Springer-Verlag Berlin Heidelberg 2008
248
rad. Additional studies are needed to find the origin of these surface electrostatic effects, which could be addressed to surface strain at cluster interfaces. Nonetheless, the synergy of EH and HAADF-STEM provides an insight into the interactions between the constituents of nanostructured systems. 1. 2. 3. 4. 5.
R Andres, T. Bein and M. Dorogi, Science, 272 (1996), p. 1323. M. Haruta, Catal. Today, 36 (1996) p.153. S. Ichikawa, T. Akita and M. Okamura, JEOL News, 38 (2003), p. 6. L. Ortolani et al., J. Eur. Ceram. Soc., 27 (2007), p. 4131 M. Wanner et al., Utramicroscopy, 106 (2006), p. 341.
Figure 1. a) Reconstructed phase map of three gold nanoparticles. b) Linescan profile and result of the numerical fit.
Figure 2. a) Linescan profile from HAADF image of a gold nanoparticles and result of the fit. b) Plot of the HAADF intensity for different particles and numerical fit.
Figure 3. a) Model for gold particles shape of decreasing dimension. b) Plot of the holographic phase shift and numerical fit showing a surface phase effect of 0.45 rad.
249
Post-Mortem investigation of Fischer Tropsch catalysts using cryo- transmission electron microscopy Dogan Ozkaya1, Martin Lok2, John Casci2 and Peter Ash1 1. Johnson Matthey Technology Centre Blounts Court Sonning Common Reading RG4 9NH UK 2. Johnson Matthey Technology Centre, PO Box1 Belasis Avenue Billingham TS231LB UK [email protected] Keywords: GTL, Fischer Tropsch, Cryo- microscopy
Co/Al2O3 catalysts are widely used in the Fischer-Tropsch, gas to liquids (GTL), catalytic reaction where syngas (CO2 and H2) is converted into higher hydrocarbon wax products. One important use of the wax product is through cracking to produce clean diesel fuel. In most production routes the catalyst is initially in the form of highly dispersed Co-oxide particles on a high surface area gamma alumina with up to 1 wt% addition of a precious metal promoter. The catalyst can then be reduced to its active state in-situ in the FT reactor or supplied in pre-reduced form. In the case of the prereduced catalyst the material is encapsulated in a wax product to prevent re-oxidation of the cobalt. Post reaction the catalyst is suspended in the wax product of the FT reaction. It is of paramount importance to analyse the initial state and the final state of a catalyst in order to understand how the reaction has progressed. Any pre or post-reactor analysis therefore needs to deal with the wax but leave the catalyst unchanged. However, the dewaxing procedures traditionally applied to the catalyst, (Soxhlet extraction and calcination at 350°C) before examination, not only partially oxidize the Co but also cause some changes in the microstructure. Consequently, the combination of Cryoelectron microscopy and cryo-microtomy offer a straightforward, but unique, route to analyse the catalyst within its original wax environment. The sample (spent catalyst had operated for 1000 hours in a slurry reactor at 210 C and 20 bar using a H2/CO ratio of 2.1) was prepared as follows: wax sample was stuck to a microtome stub using sucrose solution at liquid nitrogen temperatures and microtomed using a Leica FC-6 cryo-ultramicrotome. The slices were placed on a holey carbon coated Cu TEM grid and transferred to a Tecnai F20 field emission transmission electron microscope using a Gatan cryo-transfer system. Direct analysis of the catalyst is demonstrated with high-resolution images and analysis from the TEM. The catalyst analysed was produced using the high dispersion Catalyst (HDC) technique [1,2] rather than the more usual nitrate route. The material generated using HDC route was then reduced, generating Cobalt metal on the support, and encapsulated in wax An example of a microtomed wax on a TEM grid is shown in figure 1a. The marks from a diamond knife can be seen on the wax and this illustrates the difficulties of handling wax at low temperatures. Figure1b shows a part of the catalyst embedded
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 249–250, DOI: 10.1007/978-3-540-85226-1_125, © Springer-Verlag Berlin Heidelberg 2008
250
within the wax. It shows that diamond knife marks do not necessarily prevent the analysis of the catalyst. Figure 2a shows a region of the catalyst close up. The particle size analysis from a region like this is shown in figure 2b with catalyst as prepared (fresh) and after it has been through the reaction (spent). The changes in the particle size reflect directly the conditions that the reactor has been through and possible to correlate it with reactivity. 1. 2.
1- Lok C. M. Studies in Surface Science and Catalysis 147 (2004) 283 2- Bonne R. and Lok C. M. US patent 5, 874 (1999) 381
Figure 1. Low magnification image of the wax slice on a TEM grid (fig 1a) and a catalyst piece within a wax surround.
Figure 2. The Co metal particles on alumina support (fig 2a) with particle size distributions for a fresh catalyst and spent catalyst.
251
TEM Investigations on Cu-impregnated Zeolite Y catalysts via chloride free preparation M.-M. Pohl, M. Richter, M. Schneider Leibniz-Institute for Catalysis e.V.(branch Berlin), Richard-Willstätter-Str. 12, D-12489 Berlin, Germany [email protected] Keywords: catalysis, impregnated zeolite, Cu dispersion
Copper-containing zeolites are potential catalysts for the oxidative carbonylation of methanol to DMC [1,2] but have a minor activity without chloride. The catalyst used for this study was a chloride-free system which combines high performance with the attractiveness of a process that abandons any halogens during catalyst preparation and process operation [3]. In all those zeolite catalyst systems the question of the distribution of the copper particulary at high loading is crucial. The investigation of the complex morphologies of zeolites by microscopy is a challenge due to their beam sensitivity. Ion exchanged zeolites decrease the beam stability further. The metals leave the zeolite matrix as particles and the zeolite structures are destroyed. As ultimate consequence nanowires can be formed, shown by Mayoral and Anderson [4]. For HRTEM on zeolites the use of Cs-corrected microscopes is a suitable way Tesche [5] showed this opportunity by imaging metal clusters inside ordered pores without any loss of the 3D-Structure. Since the access on Cs-corrected microscopes are limited most microscopists have to deal with conventional TEM. The here analyzed zeolite Y with 14wt% Cu load shows the typical growth of nanoparticles under electron beam at 200kV. Even in the first seconds with intact lattice planes Cu-seeds are visible which grow further under electron bombardment. Parallel the lattice plane disappear under shrinkage of the zeolite as shown in Figure 1. Additional Cu containing particles were detected both by XRD and TEM as CuO differ considerable from the beam grown Cu features (Figure 2.). Since damage could appear within the first seconds within the microscope, no secure interpretation on fine structures of these systems should be interpreted with care . 1. 2. 3. 4. 5. 6.
S. T. King, J. Catal. 161 (1996) 530. S. T. King, Catal. Today 33 (1997) 173 M. Richter, M. Faith, R. Eckelt, E. Schreier, M. Schneider, M.-M. Pohl, R. Fricke, Applied Catalysis B.: Environmental 73(2007) 269-281 A. Mayoral, PA Anderson, Nanotechnology 18 (2007)165708(6pp) B. Tesche, F.C. Jenthoft, R. Schlögl, S. R. Bare, L.T. Nemeth, S. Valencia, A. Corma, 41. Jahrestreffen deutscher Katalytiker, Weimar 2008, P43 We kindly acknowledge the financial support by the Federal Ministry for Education and Research of the FRG, the Senate of Berlin and the European Union (project 03X2002).The sample preparation is acknowledged to Mr. R. Eckelt.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 251–252, DOI: 10.1007/978-3-540-85226-1_126, © Springer-Verlag Berlin Heidelberg 2008
252
Within 20 sec
After 1 minute
After 3 minutes
Figure 1. High-resolution at 200kV of a Cu impregnated zeolite Y (1,4 nm lattice planes) with increasing beam damage and development of Cu nano particles
Relative Intensity (%)
Zeolite Y with 14wt%Cu
100.0
CuO
* 0.0
10.0
20.0
30.0
* 40.0
50.0
2Theta
Figure 2. CuO at high Cu load detected by XRD and TEM image with CuO and beginning electron damage within the zeolite Y matrix and first Cu seeds
253
Coarsening of mass-selected Au clusters on amorphous carbon at room temperature R. Popescu1, R. Schneider1, D. Gerthsen1, A. Böttcher2, D. Löffler2 and P. Weiss2 1. Laboratorium für Elektronenmikroskopie and Center for Functional Nanostructures, Universität Karlsruhe, 76128 Karlsruhe, Germany 2. Institut für Physikalische Chemie, Universität Karlsruhe, 76128 Karlsruhe, Germany [email protected] Keywords: Au clusters growths, transmission electron microscopy, surface Ostwald ripening.
Mass-selected Aun (n=4,6,13 and 20) clusters and clusters with an initial distribution of Aum (10≤m≤20) clusters were deposited on amorphous carbon (a-C) thin films by low-energy-beam cluster deposition. The samples were stored at room temperature under ambient conditions over more than two years to analyse the stability of the cluster sizes. The cluster-size distributions were investigated by transmission electron microscopy (TEM) in regular time intervals. Several hundred Au clusters were analysed for each sample and time interval. The cluster radii were assessed by measuring the projected cluster area, which is in a good approximation a circular one. Size histograms were derived and the average radii at a given time t R (t ) were determined. Figure 1 shows the measured R (t ) values which increase strongly over a period of more than two years although the samples were not exposed to elevated temperatures. The coarsening process is best described by a least-square fit of the experimental R (t ) based on R 4 (t ) = R 4 (0) + K d t (t: time, Kd: constant), which corresponds to surface diffusion-limited Ostwald ripening (OR) with the mass transport taking place through the cluster-substrate contact line [1,2]. Coalescence of clusters caused by Brownian motion can be excluded for the given experimental conditions. The values of the surface mass-transport diffusion coefficient Ds' can be calculated using the 45 K d ln( L) ϕ (θ ) k B T , where DS' is given by Kd values and the relation Ds' = 4 ω 2 γ n0 Ds' = Ds c Au with the surface-diffusion coefficient of single Au atoms Ds on a-C and the number of single Au ad-atoms on sites of the a-C substrate cAu. ω=1.7⋅10-29 m3 denotes the volume of gold atoms, γ=1.5 Jm-2 the Au surface energy [3], n0=1.1⋅1019 m-2 the density of sites on the cluster surface [4], kB the Boltzmann constant and T=298 K the temperature. L=2.5 is the screening distance, which is taken to be constant [1]. The parameter ϕ (θ ) = 0.45 depends on the contact angle θ between the Au cluster and the a-
C substrate [4]. The Ds' values are between (1.1±0.1) and (3.8±0.4)⋅10-25 m2s-1. Values for cAu between 0.8 and 2.4⋅1017 atoms⋅m-2 can be derived for our samples as outlined in detail elsewhere [5]. The surface-diffusion coefficient of single Au atoms on a-C is
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 253–254, DOI: 10.1007/978-3-540-85226-1_127, © Springer-Verlag Berlin Heidelberg 2008
254
given by Ds (T ) = D0 exp(− Ed k BT ) with D0=1.6⋅10-8 m2s-1. Using the relation Ds' = Ds c Au with the values for cAu and Ds' , an activation energy for the surface diffusion of single Au atoms Ed=0.87±0.05 eV is determined in good agreement with a previous theoretical value of Ed=1.0 eV [6]. We show that the cAu values depend - besides on the temperature and the average distance between clusters - also on the initial Au-cluster size distribution on the substrate. They are not particularly sensitive (within our error limit) with respect to the initial size of the Aun (n=4,6,13 and 20) clusters in the case of mass-selected deposition. Moreover, the coarsening process for mass-selected Au clusters (even in case of an initial limited Au-cluster distribution) is quite different from that observed for the deposition of non mass-selected Au clusters on a-C at room temperature as reported in Ref. [7].
1. 2. 3. 4. 5. 6. 7. 8.
B. K. Chakraverty, J. Phys. Chem. Solids 28 (1967), 2401. M. Zinke-Allmang, L. C. Feldman and M. H. Grabow, Surf. Sci. 16(8) (1992), 377. W. R. Tyson and W. A. Miller, Surf. Sci. 62 (1977), 267. R. Popescu, E. Müller, M. Wanner, D. Gerthsen, M. Schowalter, A. Rosenauer, A. Böttcher, D. Löffler and P. Weis, Phys. Rev. B 76 (2007), 235411. R. Popescu, D. Gerthsen, M. Wanner, A. Böttcher, D. Löffler and P.Weiss, to be published. A. A. Schmidt, H. Eggers, K. Herwig and R. Anton, Surf. Sci. 349 (1996), 301. M. Wanner, R. Werner, G. Schneider and D. Gerthsen, Phys. Rev. B 72 (2005), 045426. This work has been performed within the project C4 of the DFG Research Center for Functional Nanostructures (CFN). It has been further supported by a grant from the Ministry of Science, Research and the Arts of Baden-Württemberg (Az: 7713.14-300).
Figure 1. a) Average radii of Au clusters as a function of storage time R (t ) . The
symbols represent the measured R for samples prepared by deposition of: Au4 (Y), Au6 ( ), Au13 (V), Au20 with 1.5⋅1012 clusters (U), Au20 with 0.75⋅1012 clusters ( ) and Aum (10≤m≤20) cluster distribution ( ). The solid lines with the corresponding colour represent fits of the data for diffusion-limited kinetics of surface OR under steady-state condition with the mass transport through the cluster-substrate contact line (see text); b) magnified section inside the dashed rectangle of a) up to 2.5 107 s .
255
TEM investigations on Ni clusters electrodeposited on Carbon substrate M. Re1, M.F. De Riccardis1, D. Carbone1, D. Wall2 and M. Vittori Antisari1* 1. ENEA, FIM Department, C.R.Brindisi, Via Appia Km 702, 72100 Brindisi- Italy * C.R.Casaccia , Via Anguillarese 301, 00123 Roma – Italy. 2. FEI, Building AAE Achtseweeg Noord 5, Acht – Eindohven 5651GG marilena [email protected] Keywords: catalysts, nanostructures, Ni clusters
The role of catalysts in the growth of carbon nanostructures by CVD is particularly critical, since the nano-carbon shape can depend on the catalyst composition and structure besides the deposition parameters [1-3]. In the synthesis of metal catalyzed carbon nanofilaments the performances of the catalyst particles can dramatically depend on both physical and chemical interaction with the substrate. In particular, a good adherence of the clusters to the substrate is necessary to avoid coalescence phenomena during the growth process generally carried out at relatively high temperature. The study of catalyst-substrate microstructure is particularly relevant for the optimization of the whole growth process. In this work Ni clusters were synthesized by electrodeposition, a versatile, rapid and inexpensive technique which, by a specific control of the process parameters, can allow the deposition of continuous metallic films or of nanoparticles, also on complex and convoluted substrates. The Ni clusters were electrodeposited on different C substrates, and have been successful used to assist the CVD growth of carbon nanofibres, having a particularly good adhesion with the substrate [4-5]. The experimental electrodeposition conditions are reported elsewhere [6]. Particularly interesting results were obtained in the case of Carbon Fibres (PAN fibres, produced by controlled pyrolysis of Polyacrylonitrile) [4-6] which were, by this method, decorated with carbon nanofibres grown at the electrodeposited Ni clusters. Transmission Electron Microscopy, with a TECNAI G2 F30 operated at 300 kV, was used to characterize the morphology and microstructure of the electrodeposited Ni and to study in detail the interface between the metal and the substrate in order to better understand the adhesion mechanism of Ni clusters to the C substrates. Considering the cylindrical shape of the Carbon Fibres, cross sectional samples for TEM observations were prepared by FIB with a FEI Strata 400 dual beam instrument. Conventional bright field and high resolution TEM images show that the Ni clusters have a globular shape, with a width in the range of 60–90 nm and a height between 50 and 80 nm (Figure 1 a). The clusters, on the contrary of a commonly observed situation, are polycrystalline and have a grain size of the order of 10 nm (Figure 1 c). The structure of the interface between the carbon substrate and the cluster is not particularly evident in the high resolution images (Figure 1 b), despite the favourable observation geometry. In order to characterize the carbon-cluster interface, EDS spectra were
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 255–256, DOI: 10.1007/978-3-540-85226-1_128, © Springer-Verlag Berlin Heidelberg 2008
256
collected with a focused electron beam. The analyses, carried out on different clusters, showed systematically a higher O content at this interface. This finding, in agreement with SIMS experiments not reported, can bring another piece of information on the interface structure and indicating the way for the interpretation of the strong bonding of the Ni clusters with the substrate. 1. 2. 3. 4. 5. 6. 7.
I. Martin-Gullon, J. Vera, J. A. Conesa, J. L. . Gonzales, C. Merino, Carbon, 44 (2006), 1572-1580 F.H. Kaatz, M.P.Siegel, D.L. Overmyer; P.P. Provencio, D.R. Talland, Appl. Phys. Lett., 89 (2006), 241915 A. de Lucas, P. B. Garcia, A. Garrido, A. Romero, J.L. Valverde, Appl. Cat. A, 301 (2006), 123-132 Th. Dikonimos Makris, R. Giorgi, N. Lisi, L. Pilloni, E. Salernitano, M.F. De Riccardis and D. Carbone, Fullerenes, Nanotubes and Carbon Nanostructures, vol 13, supplement 1 , 2005, 383-392 M. F. De Riccardis, D. Carbone, Th. Dikonimos Makris, R. Giorgi, N. Lisi, E. Salernitano, Carbon, 44 (2005) 671 M. F. De Riccardis, D.Carbone, Appl. Surf. Sci. 252 (2006), 5403-5407, We kindly acknowledge the technical support of F. Tatti, Application Specialist of FEI Italy.
Figure 1. a: a BF TEM image of the longitudinal cross section of the sample; b: a HRTEM image of the interface between a Ni cluster and the substrate; c: a HRTEM image of a small area of the Ni cluster.
257
Near-surface structure of FePt nanoparticles B. Rellinghaus1, D. Pohl1, E. Mohn1, and L. Schultz1 1. IFW Dresden, Institute for Metallic Materials, P.O. Box 270116, D-01171 Dresden, Germany b [email protected] Keywords: FePt, Nanoparticles, Aberration corrected TEM.
Stoichiometric FePt nanoparticles in the chemically ordered tetragonal L10 phase have gained significant interest in the past decade, since their huge magneto-crystalline anisotropy makes them promising materials for future ultra-high density magnetic data storage media. However, simulations of the equilibrium structure of FePt nanoparticles imply that the formation of the L10 phase may be impeded by a segregation of Pt atoms to the particle surface. Recently, an increase of the lattice constant towards the particle surface – as expected for Pt-enriched surfaces – was reported for FePt nanoparticles [1]. We have therefore systematically investigated the structure of FePt nanoparticles by aberration corrected TEM utilizing a FEI Titan3 80-300 microscope equipped with an image CS corrector (CEOS). FePt nanoparticles were prepared from the gas phase [2,3] and deposited onto amorphous carbon support films. Owing to the clean preparation process, the particle surfaces are free of any stabilizing organics. Particle morphologies and structures range from icosahedral or deceahedral multiply twinned particles (MTPs) to truncated octahedra which are often single crystals. The mean particle diameter is roughly 7 nm. Two typical FePt icosahedra are depicted in Fig. 1 where the phase of the reconstructed exit wave as obtained from the evaluation of a focus series of TEM images is shown. A detailed analysis does not reveal any systematic increase of the lattice spacing upon approaching the particle surface, but a rather statistic variation of any inter-atomic distances (not only the radial spacings). Increased lattice parameters close to the particle surface were only observed, when the particles were terminated by incomplete layers of atoms, or in the vicinity of pronounced (near-surface) defects. The latter is illustrated in Fig. 2 which shows exemplarily a truncated FePt octahedron with a near-surface edge dislocation. As can be seen from the magnification of the defected area in Fig. 2b, the spacing between the last complete (though bent) surface layer to the atoms of an additional incomplete surface layer as manifested by the faint contrast marked by the white arrows is larger than in the depth of the particle. Such defects are more likely to occur in un-equilibrated particles (see, e.g., the twin boundary in the vicinity of the sintering neck to a neighboured particle). The effect of thermal equilibration of the particles by short-time in-flight annealing will be discussed. 1. 2.
R.M. Wang, O. Dmitrieva, M. Farle, G. Dumpich, H.Q. Ye, H. Poppa, R. Kilaas and C. Kisielowski, Phys. Rev. Lett. 100 (2007) 017205. S. Stappert, B. Rellinghaus, M. Acet and E.F. Wassermann, J. Cryst. Growth 252 (2003) 440.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 257–258, DOI: 10.1007/978-3-540-85226-1_129, © Springer-Verlag Berlin Heidelberg 2008
258
3.
B. Rellinghaus, E. Mohn, L. Schultz, T. Gemming, M. Acet, A. Kowalik, and B.F. Kock, IEEE Trans. Magn. 42 (2006) 3048.
Figure 1. (a) Reconstructed exit wave (phase image) of two icosahedral FePt nanoparticles lying with their two-fold symmetry axes parallel to the electron beam. (b) Magnification of the area marked by the dashed rectangle in fig. (a). (c) Line profiles as obtained from the areas indicated in fig. (b).
Figure 2. (a) Reconstructed exit wave of a [110]-oriented truncated FePt octahedron at a focus where a near-surface edge dislocation becomes visible. The dashed line indicates a twin boundary (TB) close the sintering neck to an adjacent particle (only partly shown, bottom left corner). (b) Blow-up of the area marked in fig. (a). Dashed lines highlight the dislocation. Arrows indicate incomplete layers of surface atoms.
259
Overgrowth of gold nanorods: From rods to octahedrons J.B. Rodríguez-González, E. Carbó-Argibay, I. Pastoriza-Santos, J. Pérez-Juste and L.M. Liz-Marzán Departamento de Química Física, Unidad Asociada CSIC-Universidade de Vigo, 36310 Vigo, Spain. [email protected] Keywords: TEM, gold, nanorods.
In this work, we use transmission electron microscopy (TEM), and selected area electron diffraction (SAED) to study the growth of previously synthesized monocrystalline gold nanorods (NRs) [1]. When HAuCl4 was reduced on the rods by DMF in the presence of PVP, preferential growth on the sides was obtained, together with sharpening of the tips. TEM images of one original NR, two intermediate particles, and the final stage particle, as well the corresponding SAED patterns, are shown in Figure 1. The starting single-crystal Au NRs, are enclosed within eight {110} and {100} alternating lateral facets, whereas the rod tips are terminated by {100}, {110}, and {111} facets [2]. The SAED analysis (Figure 1) reveals that the tips of the intermediate particles are composed of four {111} facets and indicates that the lateral facets are {110}. The final particles display an octahedral shape whit all facets type {111}, while maintaining a single-crystalline structure [3]. We propose a growth mechanism as sketched in Figure 2. Transformation of the initial rods (Figure 2a) into particles with four {110} lateral facets and sharp tips enclosed by four {111} facets should involve disappearance of the {100} side facets through preferential addition of Au atoms on them (Figure 2b). The morphological transition produced by further growth of the sharp NRs will accordingly be determined by the ratio between the growth rates along the [110] and the [111] directions, this is schematically shown in Figure 2c by the red spheres closing the {110} facet and forcing the {111} facets to join, one with each other, in the final octahedral structure. The described mechanism, based on preferential growth of certain crystalline facets should correlate with a sequence of surface energies in the order {100}>{110}>{111}, which is not in full agreement with the general sequence of surface energies for the different crystallographic Au fcc planes γ(111)< γ (100)<γ(110) [4]. 1. 2. 3. 4.
B. Nikoobakht, M. A. El-Sayed, Chem. Mater. 15 (2003), 1957. Z. L. Wang, M. B. Mohamed, S. Link, M. A. El-Sayed, Surf. Sci. 440 (1999), 809. E. Carbó-Argibay, B. Rodríguez-González, J. Pacifico, I. Pastoriza-Santos, J. Pérez-Juste, L. M. Liz-Marzán, Angew. Chem. Int. Ed. 46 (2007), 8983. L. D. Marks, Rep. Prog. Phys. 57 (1994), 603.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 259–260, DOI: 10.1007/978-3-540-85226-1_130, © Springer-Verlag Berlin Heidelberg 2008
260
Figure 1. TEM images of Au nanorods in different growth steps, all particles are oriented along the [001] direction in vertical, as indicated by arrows. The corresponding electron diffraction patterns of the displayed particles, obtained in the [110] zone axis, demonstrate their single-crystalline nature; electron diffraction rotations are compensated. Scale bars: 20 nm.
Figure 2. Structural model of Au nanorods growth steps. a) Original nanorod with octagonal cross-section and {100}, {110}, {111} facets. b) Rod with sharp tips, square cross-section, {110} and {111} facets. c) Growth of a sharpened rod into an octahedral particle by deposition of Au atoms (red spheres) along the {110} facets.
261
Reactive Diffusion under Laplace Tension in Spherical Nanostructures C. Ene1, C. Nowak1, and G. Schmitz2 1. Institute of Material Physics, Univ. of Göttingen, Friedrich-Hundt-Platz 1, 37077 Göttingen, Germany 2. Institute of Material Physics, Westf. Wilhelms-Universität of Münster, Wilhelm-Klemm-Str. 10, 48149 Münster, Germany [email protected] Keywords: Laplace tension, core shell nanospheres, reactive diffusion, atom probe tomography
Nanostructures are often distinguished by complex geometries different from a planar layer structure. In order to study the influence of a spherical symmetry, as it is e.g. found in core-shell nano-spheres, thin film Al/Cu/Al and Cu/Al/Cu triple layers are deposited on substrates of 25 nm curvature radius. The thermal reaction is studied by atom probe tomography. Due to the outstanding spatial resolution and the ability to analyse three dimensional structures without projection artefacts, the growth of reaction products at the curved interfaces can be studied even on the length scale of a few nanometers. The experiments demonstrate that the reaction rate depends significantly on the deposition sequence of the metals. This observation is naturally explained by Laplace tension. Tip-shaped substrates have been prepared from tungsten wire by suitable electropolishing and subsequent field evaporation to a curvature radius of 25 to 30 nm at the apex. Triple layer systems Al/Cu/Al and also the inverse stacking sequence Cu/Al/Cu were deposited by ion beam sputtering. Single layer thickness was about 10 nm. Specimens were annealed in a UHV furnace at 110 °C for different times. After annealing, they were analyzed by atom probe tomography (see fig. 1). At both interfaces of the triple layers, the reaction of Cu and Al to a metastable Al2Cu phase is observed, and at both interfaces, these reaction develops according to a parabolic growth law. Therefore, the process is apparently controlled by diffusion across the growing product phase. However, as a most remarkable feature, we note that the width of the products at both Al/Cu interfaces are very different, although an identical reaction proceeds at identical temperature. In the case of the Cu/Al/Cu stacking, the interface close to the tip surface, the outer interface, is that of faster growth (see fig. 2). By contrast, if we chose the inverse Cu/Al/Cu stacking the inner interface is observed to be the broader one. The two growth rates differ by a factor two to three. By a quantitative model, we can show that this growth asymmetry is related to the interfacial tension, the so called Laplace tension induced by the curved interfaces, and its influence on the vacancy equilibrium at both sides of the product layer [1]. Since the diffusional transport of Cu and Al is linked to the directed transport of vacancies, a vacancy gradient necessarily accelerates or decelerates the transport across the product layer and thus the growth of the reaction product.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 261–262, DOI: 10.1007/978-3-540-85226-1_131, © Springer-Verlag Berlin Heidelberg 2008
262
1.
C. Ene, C. Nowak, and G. Schmitz, Appl. Phys. Lett. (in press)
Figure 1. (a) Electron micrograph of a layer sample deposited on a tungsten tip. (For clarity, a specimen with enlarged Al layer thickness has been chosen.) (b) Tomographic reconstruction of a typical triple layer. Each detected atom appears in the reconstruction as a grey-coded dot (Cu: light, Al: dark). Inside Cu layers, lattice planes are resolved (inset). deposition sequence 100
100
Cu concentrat on [at. %]
80 60
80
40
60
20
w
w'
0 0
5
10
15
20
40 Dc
20 w
0
5
10
w'
15 20 25 30 measurement depth / [nm]
35
40
Figure 2. Composition profile of a Cu/Al/Cu stack determined perpendicular to the interfaces after 40 min annealing at 110 °C. Inset shows the result of the opposite stacking sequence Al/Cu/Al.
263
Preparation and characterization of palladium nanoparticles with various size distributions M. Slouf1,2, H. Vlkova1, D. Kralova1 1. Institute of Macromolecular Chemistry AS CR, Heyrovskeho namesti 2, 16206 Praha 6, Czech Republic 2. Member of Consortium for Research of Nanostructured and Crosslinked Polymeric Materials (CRNCPM) [email protected] Keywords: colloids, gold and palladium nanoparticles, transmission electron microscopy
Metallic nanoparticles and their colloidal solutions in water (hydrosols) or organic solvents (organosols) have been attracting attention of scientists since 19th century [1]. Hydrosols of many metals, such as Au, Ag, Pt and Pd can be prepared either by chemical syntheses (controlled reduction of water-soluble compounds such as H[AuCl4], ref. [2]) or by suitable physical procedures (laser ablation [3], vacuum sputtering [4], etc.). Nanoparticles are employed in chemistry (catalysis, templates for further synthesis), physics (nanosensors, photophysics), biology (markers in TEM, drug carriers), polymer science (fillers of special polymers, nucleation) and in a number of other areas (medicine, industrial technology). In our previous work we developed a technique of preparation Au nanoparticles with pre-calculated size [5]. Prepared Au hydrosols were very stable and the size of nanoparticles could be varied in the range 5-200 nm. The nanoparticles were used for calibration in quantitative QELS experiments (Quasielastic Light Scattering, ref. [6]) and in laser ablation tests [3]. In the present study we try to introduce a reliable method for preparation of Pd nanoparticles with various sizes. These nanoparticles could be used for the above mentioned applications [3, 5, 6]. Moreover, we plan to employ the Au and Pd nanoparticles for testing of resolution, absorption contrast and chemical contrast in TEM and SEM microscopes equipped with special detectors. Chemical syntheses of Pd hydrosols were based on a well-established method consisting in reduction of PdCl2 with sodium citrate [7]. Our goal was to reproduce the methods described elsewhere and investigate the possibilities of obtaining Pd nanoparticles with different sizes and narrow size distributions. Emphasis was put on simplicity and reproducibility of the preparation techniques. Sizes and purity of the nanoparticles were checked by TEM, SAED and EDX. The first experiments showed that both average sizes and size distributions of Pd nanoparticles were slightly different from the literature [7]. Nevertheless, the sizes of the particles could be slightly varied (Fig. 1abc) although size distributions were somewhat broader (Fig. 1def). 1. 2.
M. Faraday, Philosophical Transactions of the Royal Society of London, 147 (1847), 145181. J. Turkevich, P.C. Stevenson, J. Hillier, Discussions of Faraday Society, 11 (1951), p. 55-75.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 263–264, DOI: 10.1007/978-3-540-85226-1_132, © Springer-Verlag Berlin Heidelberg 2008
264
3. 4. 5. 6. 7. 8.
O. Dammer, B. Vlckova, M. Slouf, J. Pfleger. Materials Science and Engineering B - Solid State Materials for Advanced Technology. 140 (2007), p. 138-146. F. Lednicky, E. Pavlova, J. Hromadkova, M. Slouf, R. Masirek. Proceedings of: Mikroskopie 2008. Nove mesto na Morave, 16.-17.2.2006. p. 35 (in Czech). M. Slouf, R. Kuzel, Z. Matej. Z. Kristallogr. Suppl. 23 (2006), 319-324. M. Slouf, J. Plestil, H. Synkova et al., Materials Structure, 12 (2005), p. 82-85. J. Turkevich, G. Kim, Science, 169 (1970), 873-879. Financial support through grants KAN200520704 (Academy of Sciences of the Czech Republic) and GACR 203/07/0717 (Grant Agency of the Czech Republic) is acknowledged.
Figure 1. Three different Pd colloids. TEM micrographs (a, b, c) and size distributions (e, f, g). Standard preparation (b, e). Diluted solutions: 2x (a, d) and 0.5x (c, f).
265
Electron microscopy for the characterization of nanoparticles D. Sommer1, U. Golla-Schindler1 1. Institute of Mineralogy, University of Münster, Corrensstr, 24, D-48149 Münster, Germany [email protected] Keywords: nanoparticles, HRTEM, SEM, STEM, EELS
The increasing use of nanoparticles in scientific and industrial applications lets the need to a better understanding into the physical and chemical properties of these particles arise. New generations of electron microscopes like field emission SEMs and energy filtered TEMs open a wide variety of applications. To investigate size, size distribution, morphology, agglomeration and chemical composition in the range of nm and the crystal structure in the range of Ǻ, we use a field emission SEM, the Zeiss 1540 EsB and a conventional JEOL 3010 operating at 297 kV equipped with a LaB6 cathode, post-column Gatan imaging filter and a 1K slow-scan CCD camera. The measurements with the SEM were performed using a special STEM detector, which allows to study conventional TEM samples and to detect the reflected signal above the sample as well as the transmitted signal simultaneously. With TEM, the structure information can be obtained by using diffraction patterns that allow to distinguish between amorphous and crystalline areas of the specimen. In addition, chemical information can be obtained by detection of X-rays with an EDX detector or electron energy loss spectroscopy (EELS) especially for light elements. The analyzed particles are produced from a wide variety of materials, e.g. gold, cobalt ferrites, cobalt, single- and multi-walled carbon nanotubes and CdSe quantum dots. The morphology, size distribution and agglomeration was obtained by taking SEM images in the conventional and transmission mode. The accuracy of the size determination can be significantly improved by using the transmission mode (Figure 1). To yield the morphological properties the nanoparticles were characterized by SEM in the conventional and transmission mode and HRTEM. Figure 2 shows an exemplary SEM image of agglomerated gold nanoparticles with different morphologies and sizes. To study crystallinity, high resolution TEM images were taken that additionally enables the measurement of the lattice spacings (Figure 3a). The chemical composition was determined by EDX and EELS (Figure 3b). 1.
We kindly acknowledge the help of Daniele Bonacchi and Fabio Franchini, who provided most of the nanoparticles and the European Comission for financial support (FP6-2004NMP-TI-4- 032731).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 265–266, DOI: 10.1007/978-3-540-85226-1_133, © Springer-Verlag Berlin Heidelberg 2008
266
Figure 1: Cobalt Ferrites a) conventional SEM image recorded with the incolumn SE detector b) image in the transmission mode (STEM) recorded with the ETD-SE detector.
Figure 2: SEM image of agglomerated gold nanoparticles with different morphologies and diagram of the size distribution.
Figure 3: a) HRTEM image of a CdSe Quantum dot. b) Electron energy loss spectroscopy of a cobalt nanoparticle.
267
Titanium dioxide nanoparticles prepared from TiOSO4 aqueous solutions J. Šubrt, J. Boháček, N. Murafa, L. Szatmáry Institute of Inorganic Chemistry, 250 68 Řež, Czech Republic [email protected] Keywords: titanium dioxide, photocatalyst, nanoparticles
Titanium dioxide nanoparticles were prepared from hydrated precursors, obtained by precipitation of TiOSO4 aqueous solutions by ammonia or alkali hydroxides under controlled conditions. The precipitation of precursors was followed by annealing of the obtained amorphous or nanocrystalline precipitates. The precipitation procedure has been carried out at constant temperature in range 090 °C and constant pH values 3, 6 or 9 either without additives or using additions of organic modification agents, like glycols, alcohols or amines. The structure and chemical composition of the precipitation products were characterized by XRD, SEM, EDS, HRTEM, SAED and XPS; IR and UV-VIS spectroscopy; and also by thermal analysis. The results demonstrated that precipitates of various crystallinity and different particle size and shape were obtained, depending on the precipitation conditions and modifiers used. The obtained precipitates were subjected to annealing under controlled conditions temperature increase rate, annealing temperature and retention time, atmosphere composition, additives used, etc. The results of XRD measurement carried out at increased temperature showed that the originally amorphous or nanocrystalline precursor when subjected to controlled annealing crystallize gradually and, depending on the annealing conditions, powders with nanocrystals size between 4 – 300 nm can be obtained. Above 800 °C presence of rutile was also observed. The starting gel and the annealing products were studied by electron microscopy (HRTEM and SEM). The results were in agreement with the XRD data and showed continuous growth of the anatase nanoparticles in the products with the heating temperature. The starting gel was formed by clusters of 5-10 nm anatase nanoparticles encapsulated within amorphous material whereas the annealing products were formed by anatase nanoparticles size of which depended on the annealing temperature and time. The anatase nanoparticles were aggregated into clusters of particles containing tens of particular nanocrystals (see Fig. 1). The HRTEM observations showed that the crystallization process can be considered as oriented coalescence of the original nanoparticles into bigger crystals. The conditions of synthesis of the initial hydrated precursor affect significantly course of the processes occurring during the annealing and also the properties of the resulting nanocrystalline TiO2. Depending on the conditions used, powders with required phase composition and crystallite size can be reproducibly synthesized. The obtained materials were tested as photocatalysts using photocatalyzed decomposition of 4-chlorophernol as model reaction. The results showed that some annealing products are
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 267–268, DOI: 10.1007/978-3-540-85226-1_134, © Springer-Verlag Berlin Heidelberg 2008
268
highly photoactive exceeding markedly the activity of the Degussa P-25 photocatalyst (see Fig. 2).
a
b
c
d
Figure 1. TEM micrographs of the TiO2 gel annealing products: a – 700 °C, 30 min; b – 800 °C, 30 min; c – 700 °C, 8 hrs; d – 800 °C, 8 hrs
Figure 2. Photocatalyzed disappearance of 4-chlorophenol. Sample 1 - starting anatase; sample 2 – 700 °C, 30 min; sample 3 – 700 °C, 8 hrs, sample 4 – 800 °C, 30 min; sample 5 – 800 °C, 8 hrs; sample 6 – 900 °C, 30 min.
269
Exploring nanoscale ferroelectricity in isolated and interacting colloidal ferroelectric nanocrystals using electron holography Daniel Szwarcman1, Yossi Lereah2, Gil Markovich1, Martin Linck3 and Hannes Lichte3 1. School of Chemistry, Raymond and Beverly Sackler Faculty of Exact Sciences, Tel-Aviv University, Tel-Aviv, Israel 2. Department of Electrical Engineering-Physical Electronics, The Iby and Aladar Fleischman Faculty of Engineering, Tel-Aviv University, Tel-Aviv, Israel. 3. Triebenberg Laboratory, Institute of Structure Physics, Technische Universität Dresden, Germany [email protected] Keywords: Ferroelectric nanocrystals, Electron holography, Piezoresponse force microscopy.
Whereas ferromagnetic nanoparticles, which form a single ferromagnetic domain, have been heavily studied and precise information exists about their magnetic properties, no such counter-part exists for nanoscale ferroelectric materials. Exchange interactions are responsible for the appearance of ferromagnetism even in small atomic clusters consisting of several Fe, Co or Ni atoms [1]. But in ferroelectric crystalline phases, it is yet to be established, what is the minimal cluster/nanocrystal size and geometry, that could support the ferroelectric crystal phase in the absence of external support such as metal electrodes or electric fields from neighbor particles. It is not even established whether a small single domain isolated nanocrystal could exist as a ferroelectrically aligned structure, because of high depolarizing fields, or that other forms of ferroelectric order should occur. Theory and modeling of such systems have been highly controversial and no detailed experimental data on ferroelectricity in small isolated nanocrystals exists. So far only polycrystalline samples and thin films of ferroelectric materials have been thoroughly studied with standard characterization techniques. Off-axis electron holography is an ideal technique for tackling such problem [2,3]. Electron holography allows the electron phase shift to be recovered. Since this phase shift can be related directly to the electrostatic potential, an electron hologram can be interpreted to provide quantitative information about electromagnetic fields with a spatial resolution approaching the nanometer scale. In this study we investigate the size effect of these isolated ferroelectric nanocrystals by electron holography. Isolated BaTiO3 nanocrystals were prepared by a molten hydroxide synthesis. The ferroelectric properties within the nanocrystals were characterized using electron holography above and below the Curie temperature, and also by Piezoresponse Force Microscopy (PFM), which can show the piezoelectric properties of the ferroelectric nanocrystals. Preliminary results from electron
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 269–270, DOI: 10.1007/978-3-540-85226-1_135, © Springer-Verlag Berlin Heidelberg 2008
270
holography experiments show (figure 1) different behavior of the polarization within different BaTiO3 nanocrystals with a strong temperature dependence on polarization. 1. 2. 3.
I.M.L Billas, A. Chatelain, W.A de Heer, Science 265 (1994), p.1682. H. Lichte, M. Lehmann, Rep. Prog. Phys 71 (2008), p.016102. H. Lichte, P. Formanek, A. Lenk, M. Linck, C. Matzeck, M. Lehmann and P. Simon, Annu. Rev. Mater. Res., 37 (2007), p.539-588. We kindly acknowledge the help of the European community. This study is supported by EC grant No. 29637.
4.
6
(a)
(b)
5 4
rad
3 2
0
5
10
15
5.0
25
30
35
(d)
10 nm 5.5
20 nm
(c)
4.5
rad
4.0 3.5 3.0
10 nm m 0
10
20
nm
30
40
50
Figure 1. Phase images of BaTiO3 nanocrystal below and above the Curie temperature. (a) at room temperature with (b) and (c) the corresponding phase linescans along (a). The phase image (d) shows the same BaTiO3 nanocrystal at 1420C.
271
STEM investigation on the one-pot synthesis of nanostructured CexZr1-xO2-BaO·nAl2O3 catalytic materials J.C. Hernandez1, J.A. Perez-Omil1, J.J. Calvino1, S. Bernal1, R. di Monte2, S. Desinan2, J. Kašpar2 and S. Trasobares1 1. Dept. de Ciencia de los Materiales e Ingeniería Metalurgica y Química Inorgánica, Universidad de Cadiz, Campus Rio San Pedro s/n, Puerto Real 11510 (Cadiz), Spain. 2. Dipt. di Scienze Chimiche, Università di Trieste, 34127 Trieste, Italy. [email protected] Keywords: STEM, CeZrO2 catalysts, one-pot synthesis
In relation with the applications of CeO2-ZrO2 mixed oxides in catalysis, new synthetic routes aim at preparing materials with improved performances in terms of durability and high temperature textural and chemical resistance [1]. Barium-doped alumina (BDA) as well as Barium hexaaluminates (BHA), BaO·6Al2O3, present high thermal stability, this making them suitable supports of highly dispersed catalytic active phases, e.g. in combustion processes [2]. Thus, these materials seem appropriate to prepare supported CeO2-ZrO2 catalysts with improved high temperature stability. In this contribution we have focused on the characterization by (S)TEM of a series of CexZr1-xO2-BaO·nAl2O3 materials prepared using a novel, one-pot, synthesis route. The goal of the characterization work was to obtain an as exact as possible picture of the distribution of the different components of these nanomaterials, as well as to characterize the chemical and structural features of all the phases involved. In order to evaluate the stability of the newly-prepared catalysts against high temperature aging, the CexZr1-xO2-BaO·nAl2O3 samples were studied after being submitted to calcination treatments at increasing temperatures up to 1200ºC. With respect to the deterioration of the catalytic response of these formulations three aspects become of major concern: (1) the formation of very large CexZr1-xO2 aggregates due to sintering; (2) the formation of large amounts of, low specific surface, BHA at the expense of large specific area BA; (3) The formation of BaO-CexZr1-xO2 or Al2O3- CexZr1-xO2 mixed phases which block the redox activity of the CexZr1-xO2 mixed oxide particles. The CexZr1-xO2-BaO·nAl2O3 samples here investigated were prepared by slow addition of a NH3 solution over a HNO3 solution containing appropriate amounts of Ba(NO3)2, Al(NO3)3, Ce(NO3)3 and Zr(NO3)4. This was followed by a treatment with H2O2 and reflux with 2-propanol for 4-6h. After filtering and washing with 2-propanol, the solid thus obtained was dried at 120ºC and further calcined at 700ºC for 5h. Hereon we will call these samples, fresh samples. HREM images of the fresh samples, Figure 1, confirmed the presence of highly dispersed, nanosized (about 7 nm), CexZr1-xO2 crystallites. In the case of samples with Ce/Zr ratios 0.2/0.8 these corresponded to the tetragonal phase. Alumina is present as γ-Al2O3, with crystal sizes about 6 nm. Increasing the calcination temperature up to 1100ºC, increased the Ce-Zr mixed oxide crystallite size. STEM-XEDS analysis in spot
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 271–272, DOI: 10.1007/978-3-540-85226-1_136, © Springer-Verlag Berlin Heidelberg 2008
272
mode indicated nevertheless that the CexZr1-xO2 crystallites did not contain Ba after calcination between 700 and 1100ºC, Figure 2. Upon calcination at 1200ºC, HREM images confirmed the formation of needle-like BHA crystals covered by a huge number of Ce-Zr mixed oxide nanocrystals, Figure 3. X-EDS element distribution maps, Figure 3, showed that Ba was preferentially incorporated into the BHA crystals. These results indicate that the synthesis route employed favours the effective separation, self-assembly, of the different components in the final material, what finally allows them expressing their intrinsic functionality. Likewise, (S)TEM appears as an essential tool to reveal the exact distribution as well as the details of the composition and structure of the different components involved in complex catalytic formulations, as those investigated in this contribution. 1. 2. 3. 4.
A. Trovarelli in “Catalysis by Ceria and Related Materials”, ed. Imperial College Press: London, 2002. G. Groppi, M. Bellotto, C. Cristiani, P. Forzatti, P.L. Villa, Appl. Catal. A, 104 (1993), 101. A.J. Zarur and J.Y. Ying, Nature, 403 (2000), 65. This works has received financial support from MEC/FEDER-EU (Proyto MAT200500333), Junta de Andalucia (FQM-110 and FQM-334) and the Ramon y Cajal 2003 Program. [010] (002) (101) (200)
5 nm Figure 1. HREM image of a sample calcined at 700ºC showing nanosized tetragonal-Ce0 2Zr0 8O2 particles.
Ba
50 nm
Al
1.1% 98.9%
Figure 2. STEM-HAADF image of a sample calcined at 1100ºC. There is no trace of Ba-CexZr1-xO2 phases.
Figure 3. STEM HAADF image and XEDS element distribution maps obtained on a sample calcined at 1200ºC
273
Enhanced stability against oxidation due to 2D self-organisation of hcp cobalt nanocrystals Isabelle Lisiecki1, S. Turner2, S. Bals2, M.P. Pileni1 and G. Van Tendeloo2 1. Laboratoire LM2N, UMR CNRS 7070, Université P. et M. Curie (Paris VI), B.P. 52, 4 Place Jussieu, F-75231 Paris Cedex 05, France 2. EMAT, University of Antwerp, Groenenborgerlaan 171, 2020 Antwerp, Belgium [email protected] Keywords: self-assembly, TEM, nanocrystals
Recently, a lot of progress has been made in understanding the changes in physical behaviour of 2D self-assembled nanocrystals and the interactive phenomena due to their long-range organisation. As atoms arranged in a different manner in solids exhibit varying physical properties, physical differences can also be expected when nanocrystals are arranged in a disordered or in a highly ordered structure. For example, the first intrinsic magnetic behaviour in fcc ordered supra-crystals of Co nanoparticles has recently been reported [1,2]. In current work, bright field transmission electron microscopy (TEM), electron diffraction (ED), high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) and energy-filtered transmission electron microscopy (EFTEM) are used to characterise cobalt nanocrystals with varying mesoscopic ordering before and after an oxidation step. Doing so, we reveal enhanced stability against oxidation due to 2D self-organisation of hexagonally close packed Co nanocrystals. The HAADF-STEM image in figure 1a shows Co nanocrystals on an amorphous carbon substrate prior to oxidation [3]. Using amorphous carbon as a substrate gives rise to both arranged areas and non-arranged/isolated particles [3]. The particles have an average size of 7.5 nm ± 0.4 nm. Electron diffraction performed on arranged and nonarranged/isolated crystals simultaneously (figure 1c) only shows sharp rings corresponding to the hcp Co structure. No oxide-shell crystal structure is detected. The absence of an oxide shell before oxidation is confirmed in figure 1b by line scans taken over the particles indicated in 1a. The particles do not show step-like intensity jumps associated with a dense core – less dense oxide shell structure. After oxidation, core-shell particles have been formed (figure 2). Electron diffraction (figure 2c) now shows an extra ring at 2.46Å, attributed to the cubic structure of CoO [4]. Therefore, the shell that has formed is CoO. Within the hexagonal arrangements the core sizes have shrunk to a size of 5 nm and an oxide shell of 1.5-2 nm has formed. The particles outside the hexagonal arrangement however have a much smaller Co core and thicker oxide shell. In most cases the crystal has even completely oxidised. This is confirmed by the line scans in figure 2b, taken of the particles indicated in 2a. The core-shell boundaries are indicated by dashed lines. The Co core of arranged particle A is larger than the core of particle B. Particle C has totally oxidised and shows a lower intensity associated with less dense CoO.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 273–274, DOI: 10.1007/978-3-540-85226-1_137, © Springer-Verlag Berlin Heidelberg 2008
274
To summarise, we show evidence of the enhanced stability against oxidation due to the 2D self-organisation of hcp Co nanoparticles. When the particles are ordered, they favour the formation of core-shell Co-CoO nanostructures, whereas nanocrystals in disordered arrays or isolated on the substrate are found to oxidise completely to CoO.
Figure 1. Co nanocrystals before oxidation: a) HAADF-STEM image showing hexagonally arranged and isolated particles; b) Line scan intensity profiles over the particles indicated in a). No core-shell intensity step is visible; c) SAED pattern of arranged and isolated particles showing only rings corresponding to hcp Co.
Figure 2. Co nanocrystals after oxidation: a) HAADF-STEM image showing arranged particles with core-shell structure and isolated particles with smaller core (larger shell) or totally oxidised particles; b) Line scan intensity profiles over the particles indicated in a). The isolated particles have a smaller core or have been totally oxidised compared to the arranged particles; c) Electron diffraction pattern of arranged and isolated particles together showing hcp Co and cubic CoO rings. 1. 2. 3. 4. 5.
I. Lisiecki, P.A. Albouy, M.P. Pileni, Adv. Mater., 2003, 15, 712 I. Lisiecki, D. Parker, C. Salzemann, M.P. Pileni, Chem. Mat., 2007, 19, 4030. I. Lisiecki, C. Salzemann, D. Parker, P.A. Albouy, M.P. Pileni J. Phys. Chem. C, 2007, 111, 12625. I. Lisiecki, M. Walls, D. Parker, M.P. Pileni Langmuir, 2008, (In press) This work has been performed within the framework of IUAP P5/01 of the Belgian government
275
Loaded porous Zn4O(bdc)3 (metal@MOF-5) frameworks characterised by TEM S. Turner1, O.I. Lebedev1, F. Schröder2, R.A. Fischer2 and G. Van Tendeloo1 1. EMAT, University of Antwerp, Groenenborgerlaan 171, 2020 Antwerp, Belgium 2. Anorganische Chemie II – Organometallics & Materials, Ruhr-Universität Bochum, Universitätsstrasse 150, D-44780, Germany [email protected] Keywords: Metal@MOF-5, TEM, Electron Tomography
In recent years, metal-organic frameworks (MOFs) have received much attention because of their high specific surface areas and pore volumes, applicable in gas storage, catalysis, and photovoltaics [1]. Recently, Zn4O(bdc)3 (MOF-5; bdc = 1,4 benzenedicarboxylate) crystals have been loaded with catalytically active material like Pd, Au, Cu and Ru leading to a heightened catalytic activity in olefin hydrogenolysis and methanol synthesis [2]. These metal@MOF-5 materials can be produced by gasphase loading of metal-carrying precursors into the MOF-5 framework. This loading procedure is known to yield a MOF-5 framework loaded with catalytically active nanoparticles in the range of 1-3 nm [3]. The local distribution of these particles within the MOF-5 framework however remains unclear. Furthermore, MOFs are known to be chemically labile and the loading procedure may affect the framework structure. We show that by minimising the electron dose to avoid beam damage [4], transmission electron microscopy (TEM) can be used to characterise this new family of soft materials on a local scale. Bright field TEM and electron diffraction (ED) are used to provide structural information on the metal@MOF-5 crystals. High-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) imaging aids easy recognition of the particles. The spatial distribution of the metal particles throughout the MOF matrix is visualised using electron tomography. Figure 1a shows a bright field TEM image of Pd@MOF-5. The MOF-5 crystals are clearly faceted; a first indication that the metal organic framework is intact after gasphase loading. The embedded Pd particles (inset) have sizes ranging from 1-5 nm, in good agreement with the metal@MOF-5 model [3]. In the HAADF-STEM image in 1b the Pd particles (bright white contrast) appear to be spread throughout the MOF. The diffraction patterns in 1c and 1d show the cubic structure of the MOF-5 matrix, confirming that the framework remains intact. The faint ring in 1d at 2.25Å corresponds to the crystalline Pd particles. Figure 2a displays a typical Pd@MOF-5 crystal with embedded Pd particles up to 5 nm visible (inset). Some agglomerates are present, possibly indicating a local collapse of the MOF. In 2b, the tomographically reconstructed particles are imaged. Figure 2c is a slice taken through the tomographically reconstructed MOF-5 volume. Electron tomography can clearly distinguish between particles within the MOF and particles on the surface. In the present case, the Pd particles are spread throughout the MOF-5 matrix, and are not preferentially found at the surface of the crystals. S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 275–276, DOI: 10.1007/978-3-540-85226-1_138, © Springer-Verlag Berlin Heidelberg 2008
276
Figure 1. Palladium@MOF-5: a) Bright field TEM image showing a faceted MOF. Inset: Pd particles in the MOF; b) HAADF-STEM image; c) Diffraction pattern of the cubic MOF-5 framework in [001]* zone axis; d) Diffraction pattern of the framework in [-223]* zone axis and a ring corresponding to the 111 spacing in cubic Pd.
Figure 2. Palladium@MOF-5: a) Bright field TEM image; b) Tomographic reconstruction of the Pd-particles in the MOF-5 matrix; c) Slice taken through the reconstructed volume of the MOF-5 crystal. The metal particles are spread throughout the MOF, although some surface agglomerates are present. 1. 2. 3. 4. 5.
Li, H.; Eddaoudi, M.; O’Keeffe, M; Yaghi, M., Nature 1999, 402, 276-279. Hermes, S et al., Angew. Chem., Int. Ed. 2005, 44, 6237-6241 Schröder F. et al., JACS 2008, (In press) Lebedev, O.I. et al., Chem. Mater. 2005, 17, 6525-6527. The authors acknowledge support from the European Union under the Framework 6 program under a contract from an Integrated Infrastructure Initiative (Reference 026019 ESTEEM)
277
Growth behaviour of sub-nm sized focused electron beam induced deposits W.F. van Dorp 1,3, C.W. Hagen1, P.A. Crozier2, P. Kruit1, S. Zalkind3, B. Yakshinskiy3 and T.E. Madey3 1. Delft University of Technology, Lorentzweg 1, 2628 CJ Delft, Netherlands 2. School of Materials, Arizona State University, Tempe, AZ, 85287 3. Laboratory for Surface Modification, Rutgers University, Piscataway, NJ, 08854 w f.vandorp@tudelft nl Keywords: nanometer scale, FEBIP, EBID
Developing techniques for the controlled fabrication of nanostructures is a topic of intense research and is critical to exploit the full potential of nanotechnology. Focused electron beam induced deposition (EBID) is a versatile, direct, and resistless fabrication technique [1, 2]. Precursor molecules, introduced into a vacuum chamber, adsorb on the substrate and are dissociated into fragments under the influence of a focused electron beam. The fragments of the precursor molecules stick to the surface and form a deposit. We performed our EBID experiments in an environmental Scanning Transmission Electron Microscope (STEM) with a beam energy of 200 keV, a 0.3 nm probe, W(CO)6 as a precursor gas and amorphous carbon as a substrate. Typical precursor gas pressures during the deposition were 10-3 Torr, and the sample was held at 150 ˚C to reduce contamination from the microscope. We used the annular dark field (ADF) signal for the imaging of the deposits. By recording the ADF signal during deposit growth, we were able to monitor the growth process in situ. Additionally, atomic force microscope measurements were performed on the deposits to determine the volume of the deposits. We deposit arrays of dots (Fig. 1). The smallest deposits we have been able to fabricate have an average full width at half maximum of 0.7 nm [3]. These are the smallest EBID deposits reported to date and at this small scale, the process is not linear anymore. Although all deposits in the array are created with a fixed dwell time, the amount of mass varies from deposit to deposit. This can be seen in Fig. 1 as a variation in intensity in the ADF image. The distributions of mass become relatively wider as the dwell time decreases and the deposits contain less material. The distributions of mass bear close a close resemblance to Poisson distributions (Fig. 2). This indicates that each of the deposits consists of a discrete number of units. The volume of these units was determined by fitting Poisson distributions to the experimental data and combining this with the AFM measurements and was found to be 0.4 nm3. Our work on EBID continues with a study of the adsorption and dissociation chemistry of CH3-Pt-C5H4CH3 on Au(110). Fig. 3 shows results from temperature programmed desorption (TPD) measurements. The first monolayer in contact with the substrate has a higher desorption temperature and a correspondingly higher adsorption energy than condensed multilayers. We plan to use TPD measurements to determine the cross section for electron beam induced dissociation as a function of electron energy.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 277–278, DOI: 10.1007/978-3-540-85226-1_139, © Springer-Verlag Berlin Heidelberg 2008
278
1. 2. 3.
S.J. Randolph, J.D. Fowlkes, P.D. Rack, Crit Rev Solid State Mater Sci 31, (2006) 55 W.F. van Dorp, B. van Someren, C.W. Hagen, P. Kruit, P.A. Crozier, Nano Lett 5, (2005) 1303 W.F. van Dorp, C.W. Hagen, P.A. Crozier, P. Kruit, J Vac Sci Technol B 25 (2007), 2210
Figure 1. ADF image of an array of deposits created with EBID. The dwell time of the e-beam per deposit is identical for all deposits. 140e-9 Torr
B
48e-9 Torr
250
36e-9 Torr λ=1
18e-9 Torr 12e-9 Torr
150 100
0.4
24e-9 Torr
200
6e-9 Torr
A
0.3 Probability
Intensity for m/z = 39 (arb. units)
300
λ=2 λ=3
0.2
λ=5
λ=8
0.1
50 0
0 -150
0
-100 -50 0 Temperature (Celsius)
50
Figure 3. Preliminary results from TPD measurements of CH3-Pt-C5H4CH3 on Au(110). The curves represent the rate of desorption as function of temperature for different gas doses (100s exposure at the indicated pressures). Peaks marking the first monolayer (A) and multilayers (B) are indicated.
5
k
10
15
20
Figure 2. (a) Mass distributions for deposits created with different dwell times. Deposit intensities are measured from ADF images. Negative values are due to the image processing. (b) Another set of data, similar to (a), but with deposit intensities converted to volumes using an AFM measurement. (c) Poisson distributions for expectation values (λ) of 1, 2, 3, 5 and 8. The Poisson distributions are similar to the experimental data.
279
Ruthenium deposition on CO2 -treated and untreated carbon black investigated by electron tomography M. Wollgarten, R. Grothausmann, P. Bogdanoff, G. Zehl, I. Dorbandt, S. Fiechter and J. Banhart Helmholtz Centre Berlin for Materials and Energy (formerly Hahn-Meitner-Institute) Glienicker Str. 100, D-14109 Berlin, Germany [email protected] Keywords: Ru catalysts, electron tomography
Ruthenium nano-particles modified by selenium were investigated in the last decade as an alternative to platinum which is used as electro-catalyst in fuel cell cathodes. In order to achieve highly loaded Ru-Se catalysts in a well dispersed and active state, selected parameters of the preparation procedure were optimised, such as the morphology and surface chemistry of the carbon support, the active metal precursor compounds, the amount of the selenium promoter and the process parameters of the thermal treatment during catalyst formation [1]. These investigations revealed, that the characteristics of the carbon blacks used differ significantly and have a severe impact on the distribution and size of the ruthenium particles. The role of the carbon black pretreatment by CO2 on the ruthenium deposition properties is investigated in this contribution. Commercial carbon black (Black Pearls by Cabot and Vulcan XC-72 by Cabot) was used as starting material, which was either used as-received or pre-treated in a CO2 atmosphere at a temperature of 950 °C. Ruthenium loading was done by impregnation with RuCl4 and a subsequent heat treatment at 250°C in a H2/N2 atmosphere. Finally, the carbon-supported ruthenium nanoparticles were modified with selenium by impregnation with SeCl4 and a heat treatment at 850°C. Differences in porosity of the carbon support and the distribution of RuSex particles are investigated by TEM tomography in a Zeiss LIBRA 200 microscope. Reconstructed volume data sets are obtained using the IMOD [2-3] software for reconstruction of tilt series. Figure 1 shows typical examples for the observed morphologies: Vulcan XC-72 carbon black has less porous parts on which large catalyst particles are deposited, whereas Black Pearl carbon black has a fine porosity with small and uniformly distributed Ru-particles. 1. G. Zehl, G. Schmithals, A. Hoell, S. Haas, C. Hartnig, I. Dorbandt, P. Bogdanoff, S. Fiechter, Angewandte Chemie / International Edition 46 (2007) p. 7311-7314 2. J. R. Kremer, D.N. Mastronarde, J.R. McIntosh, J. Struct. Biol. 116 (1996) p. 71-76. 3. D. N. Mastronarde, J. Struct. Biol. 120 (1997) p. 343-352. 4. The work present here is part of the project Application Centre for Tomographic Methods in Material Science and is cofinanced by the European Union and the City State of Berlin.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 279–280, DOI: 10.1007/978-3-540-85226-1_140, © Springer-Verlag Berlin Heidelberg 2008
280
(a)
(b) Figure 1. Reconstructions of a limited tilt series images obtained by TEM tomography of Ru-Se catalysts (white) on CO2 treated soot (dark grey), (a) Vulcan XC-72 and (b) Black Pearls. Differences in the morphology of both carbon supports as well as in distribution and size of the Ru-particles are clearly visible (grid spacing 20 nm).
281
Size-dependent crystallinity and relative orientations of nano-Pt/γ-Al2O3 J.C. Yang1, L. Li1, S. Sanchez2, J.H. Kong2, Q. Wang3, L.L. Wang2, Z. Zhang1, D.D. Johnson2, A.I. Frenkel3, R.J. Nuzzo2 1. Mechanical Eng. & Materials Sci., University of Pittsburgh, 848 Benedum Hall, Pittsburgh, PA, USA 2. Chemistry, Univ. of Illinois at Urbana-Champaign, 505 S. Matthews Ave., Urbana, IL, USA 3. Physics, Yeshiva University, 2495 Amsterdam Ave, Suite 501, New York, NY, USA [email protected] Keywords: Pt, heterogeneous catalysis, nanoparticles, γ-Al2O3
Platinum nanoparticles (NPs) on γ-Al2O3 support is a popular active catalytic system. Recently, in situ X-ray Absorption Spectroscopy (XAS) measurements of this system showed negative thermal expansion, where the nearest neighbor Pt-Pt bond distances decreased with increasing temperature. The unusual phenomena must involve the charge transfer interactions between the Pt particle and the γ-Al2O3 support. Preliminary theoretical simulations revealed that the energetically favorable Pt nanoparticle structures, including their bond-lengths, depend quite sensitively on orientation, surface structure and defects on the γ-Al2O3 surface. For example, O vacancies tend to pin the Pt nanoparticle and significantly change their structure, including a decrease of their bond-lengths with increasing temperatures. Therefore detailed knowledge of the atomic structure of both Pt particles and γ-Al2O3, as well as their structural correlations, is needed. Although high-angle annular dark-field (HAADF) technique is widely used in imaging heterogeneous catalytic materials because of the high contrast of the heavy metal relative to the low-Z support, the information from the support is limited, see Fig. 1. Phase contrast given by highresolution transmission electron microscopy (HRTEM) provides sub-nano information of both the Pt and γ-Al2O3 simultaneously. The samples were prepared by impregnating the Pt2+ precursor, Pt(NH3)4(OH)2⋅H2O, on γ-Al2O3, reducing in H2 gas at 573 K in order to remove the ligands to form metallic nanoparticles. The sizes of Pt particle were controlled by the loading amount, where 1 wt% produced an average Pt sizes of ~1nm and heavy loading of 5 wt% produced sizes of ~2.9 nm. The TEM samples were prepared by spreading a drop of Pt/γ-Al2O3 suspension in ethanol onto an ultra-thin Cgrid, naturally dried. The HRTEM observations were carried out with JEM 2100FEG S/TEM, operated at 200 kV. Fig. 2 is an HRTEM image taken from the 1 nm Pt sample. We noted that the crystallinity of the Pt particles is size-dependent. The 1 nm Pt particles or smaller did not show clear evidence for crystallinity. The lack of uniform bond-lengths and order is supported by XAS and theoretical simulations. The 2.9 nm Pt sample showed fcc structure with a = 0.39 nm, where a few particles contained twin boundaries. The HREM image in Fig. 3 is selected to show orientation correlation of a
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 281–282, DOI: 10.1007/978-3-540-85226-1_141, © Springer-Verlag Berlin Heidelberg 2008
282
Pt particle with its support. The Pt particle with [110] zone axis located on the γ-Al2O3 with [100] axis, rotated with an angle of ~25.5° between Pt (002) and γ-Al2O3 (004) planes. The mis-orientation of Pt particles on γ-Al2O3 suggests weak interfacial interaction of Pt/γ-Al2O3 system. This research is funded by Department of Energy – Basic Energy Sciences (DE-FG02-03ER15476). The TEM characterizations were carried out at Nanoscale Fabrication and Characterization Facility (NFCF) at the University of Pittsburgh.
Figure 1. HAADF image of Pt particles with an average size of ~2.9 nm.
Figure 2. HREM image of Pt particles and γ-Al2O3. The average size of Pt particles is ~0.9 nm.
Figure 3. HREM image of a Pt [110] particles on γ-Al2O3 [100]. (b) and (c) are FFT from the Pt particle and γ-Al2O3, respectively.
283
Formation of nanometer-sized porous GaSb particles by vacancy clustering induced by electronic excitation H. Yasuda1, A. Tanaka1, N. Nitta1, K. Matsumoto1 and H. Mori2 1. Department of Mechanical Engineering, Kobe University, Kobe 657-8501, Japan 2. Research Center for Ultra-High Voltage Electron Microscopy, Osaka University, Suita, Osaka 565-0871, Japan [email protected] Keywords: nanoparticle, structural change, electronic excitation
Porous materials play an important role for developments of luminescent, catalytic, hydrogen storage materials and so on, in which the properties can be greatly improved by a large surface-to-volume ratio. If we can prepare a porous structure not only in the bulk materials but also in the interior of individual nanoparticles, it is expected that the porous structure increases the surface area of the nanoparticles. We found that phase changes take place by atom displacements when GaSb semiconductor compound nanoparticles are excited by electron beam [1,2]. In the present work, the formation of porous semiconductor GaSb compound nanoparticles by clustering of vacancies introduced efficiently by electronic excitation and the formation mechanism has been studied by in situ TEM. Preparation of size-controlled GaSb particles was carried out with the use of a double-source evaporator installed in the specimen chamber of a TEM. Electronic excitation experiments and observations were carried out using the same microscope. The TEM used was Hitachi H-7000 operating at an accelerating voltage of 25 kV. The value of electron flux used for excitations was approximately 1.0x1020 e m-2s-1. The temperature of the supporting films was kept at 430 K. Structural changes associated with excitations were observed in situ. An example of the structural changes in GaSb particles by electronic excitation is shown in Fig. 1. Figures 1(a) and (a') show a BFI of particles with the mean diameter of approximately 20 nm before excitation and the corresponding SAED, respectively. As indexed in Fig. 1(a'), the Debye-Scherrer rings can be consistently indexed as those of GaSb which has the zincblende structure. The same area after excitation for 60 s is shown in Fig. 1(b). In the interior of the particles after the excitation, there appear voids with bright contrast. As seen from a comparison of the magnified images Ia and IIa in (a) with Ib and IIb in (b), the diameter of nanoparticles after the excitation increased up to 15 % compared with those before excitation. In the SAED taken after the excitation as shown in Fig. 1(b'), Debye-Scherrer rings of the zincblende structure are recognized again, but the lattice constant increased up to 1.8 % compared with that before excitation. The same area after excitation for 480 s is shown in Fig. 1(c). The voids in the individual particles change in the shape and size, as seen from a comparison of the magnified images Ib and IIb in (b) with Ic and IIc in (c). In the SAED taken after the excitation as shown in Fig. 1(c'), Debye-Scherrer rings are recognized, superimposed on
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 283–284, DOI: 10.1007/978-3-540-85226-1_142, © Springer-Verlag Berlin Heidelberg 2008
284
a weak halo ring. The Debye-Scherrer rings can be indexed consistently as those of crystalline antimony, which has the hexagonal structure. The value of the scattering vector (K= (4πsinθ)/λ) for the halo ring is approximately 31.0 nm-1 which is corresponding to the first halo of liquid gallium. This result indicates that a two-phase mixture consisting of a crystalline antimony core and a liquid gallium shell was formed in the particles. From these results, it has been evident that when GaSb particles kept at 430 K are excited by 25keV electrons, two-phase separation takes place via void formation. In this case, it is considered that gallium atoms on the lattice points are displaced by the electronic excitation to form vacancies and gallium interstitials in the crystal. Fig. 2 shows schematic illustrations of defect migrations and defect concentrations as a function of distance from the center of a nanoparticle and the structural changes. The vacancy concentration in the particle core is higher than that in the surface layer, but interstitial concentration increases toward the surface. Consequently, under the condition of vacancy supersaturation in the particle core the vacancy clusters will grow to form a void, and the subsequent surface segregation of interstitial clusters will bring about the separation to the two-phase structure. 1. 2.
H.Yasuda, H.Mori, J. G. Lee, Phys. Rev. Lett. 92 (2004), p.135501. H. Yasuda, H. Mori, J. G. Lee, Phys. Rev. B 70 (2004), p.214105.
~20nmφ
Defects concentration
Figure 1. An example of the structural changes in GaSb particles kept at 430 K by electronic excitation. (a)(a') before excitation, (b)(b') after 60 s, (c)(c’) after 480 s. Vacancy Interstitial
Surface layer
Void
Vacancy
Gallium antimonide
Interstitial
Void formation
Void Antimony Gallium
Phase separation
Figure 2. Schematic illustrations of defect migrations and defect concentrations as a function of distance from the center of a nanoparticle and the behaviors of the structural changes.
285
Structural investigations of membrane electrode assemblies in fuel cells via environmental scanning electron microscopy S. Zils1, N. Benker2 and C. Roth1 1. Institute for Materials Science, Technische Universität Darmstadt, Petersenstr. 23, 64287 Darmstadt, Germany 2. Institute of Applied Geosciences, Technische Universität Darmstadt, Schnittspahnstraße 9, 64287 Darmstadt, Germany [email protected] Keywords: ESEM, PEMFC, membrane electrode assembly, degradation, quasi in-situ structure research
The ideal membrane electrode assembly (MEA) for polymer electrolyte membrane fuel cells (PEMFC) would combine an improved accessibility of the noble metal catalysts with a good electronic contact of the ion- and electron-conducting parts of the fuel cell. To investigate the contact between these ion- and electron-conducting parts, so far detailed studies have only been performed by using Scanning Electron Microscopy (SEM) and Transmission Electron Microscopy (TEM) [1], which exclude the investigation of the MEA under realistic conditions. In this work, environmental scanning electron microscopy (ESEM) is used in order to obtain significant information of the structure under quasi in-situ conditions. This technique allows for studying the membrane electrode assemblies under different gas atmospheres as well as in different relative humidities and temperatures. These aspects render the possibility to adjust conditions in the sample chamber similar to a working fuel cell. Membrane electrode assemblies with a noble metal loading of 1.6 mg cm-2 have been manufactured by using an airbrush technique first described by Wilson and Gottesfeld [2]. Nafion® 117 (DuPont) has been applied as proton conducting membrane. On both the anode and the cathode side carbon-supported platinum catalysts (20 wt% on carbon black) have been used as electrodes. Sample preparation for ESEM was performed by cutting slices with a size of 2 mm by 10 mm out of the MEA. The ESEM measurements were carried out with a Quanta 200 F (FEI company, Netherlands) equipped with a field emission gun (FEG) and an energy dispersive X-ray (EDX) detector for elemental analysis. The pressure in the sample chamber can be increased in steps of 0.01 mbar, while the temperature of the sample can be varied in steps of 0.1 K using a Peltier element. For the quasi in-situ experiments a temperature of 5 °C was maintained. The pressure in the chamber and therewith the relative humidity (RH) were increased stepwise from 0.5 mbar corresponding to a RH of about 5 % up to a pressure of 8.7 mbar and a RH of 100 % at 5 °C, respectively. Figure 1 shows a sequence of two ESEM micrographs of a MEA cross section. The left image shows the cross section of the MEA at a relatively low pressure of 0.5 mbar.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 285–286, DOI: 10.1007/978-3-540-85226-1_143, © Springer-Verlag Berlin Heidelberg 2008
286
From this starting point the pressure in the sample chamber was increased stepwise and a swelling of the membrane electrode assembly could be discovered. First droplets on the membrane surface were observed at a RH of about 20 %, first droplets on the electrode surfaces at a RH of about 35 %.
Figure 1: Secondary electron images of a MEA cross section at 0.5 mbar (~ 5 % RH) and at 3.11 mbar (~ 36 % RH). The MEA swelled due to the chemical properties of the perfluorinated polysulfonic acid Nafion® until the maximum content of water in the membrane was reached. The droplets on the surface of the electrodes started to grow only after this point was reached. We expect that the comparison of a reference MEA with a MEA, which has been running in a long-term single cell test, will give us valuable insight into the interface between the electrodes and the proton-conducting membrane as well as about the effect of water at this interface. At long sight, we might even be able to investigate the cold start behaviour of polymer electrolyte fuel cells quasi in-situ and achieve significant information for an optimized fabrication of membrane electrode assemblies. 1. 2.
F. Scheiba, N. Benker, U. Kunz, C. Roth and H. Fuess, J. Power Sources 177 (2008), p. 273. M. S. Wilson and S. Gottesfeld, J. Electrochem. Soc. 139 (1992), p. 1.
287
In situ TEM nanocompression testing A.M. Minor1, J. Ye1 and R.K. Mishra2 1. National Center for Electron Microscopy, Lawrence Berkeley National Laboratory, Berkeley, CA USA 2. General Motors Research and Development Center, Warren, MI USA [email protected] Keywords: in situ TEM, mechanical properties
Recent progress in small-scale mechanical testing methods has greatly improved our understanding of size effects in volumes of a few nanometers to a few microns [1-5]. Besides the important results related to the effect of size on the strength of small structures, the ability to systematically measure the mechanical properties of small volumes of material allows us to test samples that cannot easily be processed in bulk form. Recently, we have used a quantitative in situ TEM mechanical testing device to compress microfabricated pillars inside a TEM so that we can make a direct correlation between an imposed stress and an individual deformation event. This talk will demonstrate how individual microstructural features can be tested directly with this technique, allowing us to explore the fundamental origins of strength and ductility through dynamic observations of plasticity in metallic systems (see Figures 1 and 2). Specifically, results will be presented where the in situ experiments give us some insight into the size effects seen in ex situ pillar compression tests. In addition to the studies of size effects in nanoscale volumes, the in situ nanocompression technique has allowed us to probe the fundamental origins of ductility in complex metallic alloys. As an example of this latter capability, two AA6063 alloys with identical compositions were studied for comparison, one as-extruded and the other heat treated to increase the solute concentration in the matrix. By performing in-situ nanocompression tests on microfabricated pillars we found that the annealed sample exhibited a higher yield stress and greater nanoscale ductility as compared to the as-extruded sample, analogous to what is seen through bulk mechanical testing. Furthermore, our dynamic observations and comparison of the two alloys demonstrate that the dislocation plasticity behavior is quite different for the two samples. The annealed sample showed a complex three-dimensional deformation behavior due to extreme dislocation entanglement, whereas the as-extruded sample showed a simpler two-dimensional plasticity composed of mostly planar slip behavior. This difference in behavior was attributed to the lowered stacking fault energy and thus decreased cross-slip in the annealed alloy. Our observations suggest that achieving a more complex threedimensional plasticity at the nanoscale can be directly correlated to increasing the ductility in a bulk alloy. Demonstrating the power of this new in situ mechanical testing capability, we have successfully correlated the bulk mechanical behavior of a complex alloy with its nanoscale plasticity.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 287–288, DOI: 10.1007/978-3-540-85226-1_144, © Springer-Verlag Berlin Heidelberg 2008
288
1. 2. 3. 4. 5. 6.
Uchic, M.D., Dimiduk, D.M., Florando, J.N. & Nix, W.D. Sample dimensions influence strength and crystal plasticity. Science 305, (2004), p. 986-989. Greer, J.R., Oliver, W.C. & Nix, W.D. Size dependence of mechanical properties of gold at the micron scale in the absence of strain gradients. Acta Mater 53, 1821-1830 (2005).F. Author, S. Author and T.H. Author, Journal volume (year), p. 1. Volkert, C.A. & Lilleodden, E.T. Size effects in the deformation of sub-micron Au columns. Philos Mag 86, 5567-5579 (2006). A.M. Minor, Z.W. Shan, E.A. Stach, S.A. Syed Asif, E. Cyrankowski, T.J. Wyrobek, and O.L. Warren, "A new view of the onset of plasticity during the nanoindentation of aluminum", Nature Materials, 5, (697-702) 2006 Z.W. Shan, R.K. Mishra, S.A. Syed Asif, O.L. Warren and A.M. Minor, “Mechanical annealing and source-limited deformation in submicron-diameter Ni crystals”, Nature Materials, 7 (115-119) 2007 This research was supported by the Scientific User Facilities Division of the Office of Basic Energy Sciences, U.S. Department of Energy under Contract # DE-AC02-05CH11231 and the General Motors Research and Development Center.
Figure 1. Low magnification TEM image showing in situ nano-compression experimental setup. The flat diamond punch can be seen in the upper right, approaching the top of the pillar structure on the left.
Figure 2. In situ nanocompression test of a AA6063 alloy micropillar. (a) The pillar before compression, (b) stress vs. displacement data from the in situ test, (c) the pillar after compression.
289
Physical measurements on an individual nanostructure in a TEM nanolaboratory M. Kobylko1, S. Mazzucco1, R. Bernard1, M. Kociak1, C. Colliex1 1. Laboratoire de Physique des Solides, UMR CNRS 8502, Bât. 510, Université Paris-Sud 11, F-91405 Orsay, France [email protected] fr Keywords: in situ microscopy, transport measurements, dedicated specimen holders
With the rapidly growing development in nanosciences, the requirement for realizing physical measurements on well-identified and -characterized individual nanostructures has become unavoidable to complement the vision brought by average measurements on an ensemble of insufficiently characterized nanostructures. A TEM column offers the right environment to explore this approach. It is as more of present concern as two factors favour this technical development: (i) the limited available space between the objective lens pole piece gap has been relaxed with the introduction of Cs correctors in the TEM column (as an example a probe size diameter of 0.1nm is achieved in a SuperSTEM Nion column with a 4mm gap); (ii) advances in microtechnology has made the miniaturization of actuators and sensors more widely available. Within this global context, we have become fully convinced that the design and fabrication of in situ devices is a priority for preparing the way towards a more comprehensive use of future TEM. These instruments should offer all components of a nanolaboratory, where the experimentalist can chose a nanostructure of given size, dimension, structure and composition as the object to be studied during application of an external constraint such as an electric, a magnetic or an electromagnetic field. In this contribution, our intent is to illustrate how we approach this goal by designing and using in situ transport and nanomanipulation TEM sample holders, following some of the trends already explored by Olin and co-workers [1]. The first one is targeted for simultaneous observation / structure determination and electrical transport measurements on on chip nanoobjects (Figure 1a). The second one allows simultaneous observation / structure determination, electrical transport measurements and mechanical manipulation of nanoobjects placed on tips (Figure 1b). Other devices have been built for in situ detection (or illumination) of light from or on a given area of a nanostructure [2]. These in situ TEM-holders pave the way to new meaningful experiments. For example, using a home-made TEM holder of type 2, we could monitor the process of dipping individual CNTs into mercury droplets. Such experiments are intended to measure the transport properties of individual CNTs (ballistic or diffusive behaviour, conductance quantification, etc). Our in situ experiments show that the measurement of conductance quantification in CNTs can be related to the formation of Hg-nanocontacts (Figure 2) and not to an intrinsic property of the CNTs, as suggested by earlier studies [3]. In addition, elastic medium theory simulations reveal that, when CNTs of small radii or made of few walls are considered, the probability that the CNT
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 289–290, DOI: 10.1007/978-3-540-85226-1_145, © Springer-Verlag Berlin Heidelberg 2008
290
actually enters the drop of mercury is very small [4]. These are only first results confirming the importance of developing the “nanolaboratory” approach within a TEM column, but there is no doubt that many others will rapidly follow. 1. 2. 3. 4.
K. Svensson, et al., Review of Scientific Instruments 74 (2003), 4945. See Mazzucco et al, these conference proceedings. S. Frank, P. Poncharal, Z.L. Wang and W.A. de Heer, Science 280 (1998), 1744. M. Kobylko, M. Kociak, et al., to be published (2008).
(a)
(b)
Figure 1. TEM-holders for in situ TEM measurements: (a) Transport holder for simultaneous electrical transport measurements and structure determination/observation of on chip nanoobjects; (b) Nanomanipulator holder for simultaneous electrical transport measurements, structure determination/observation and mechanical manipulation of nanoobjects on tips.
Figure 2. In situ measurement of the conductance between a tip decorated with CNTs and a mercury droplet, demonstrating the role of Hg-nanocontacts. When performed ex situ, this experiment would have wrongly attributed the measured conductance to the ballistic nature of the transport properties of CNTs.
291
TEM study of nanostructured BZO templates in (001)-LAO and (001)-STO substrates for the growth of superconducting YBCO films P. Abellan1, M. Gibert1, F. Sandiumenge1, M.J. Casanove2, T. Puig1 and X. Obradors1 1. Institut de Ciència de Materials de Barcelona, CSIC, 08193 Bellaterra, Spain 2. CEMES, 29 rue Jeanne Marvig, BP 94347, 31055 Toulouse Cedex 4, France [email protected] Keywords: YBCO, BZO, CSD
A methodology for the preparation of artificially nanostructured oxide templates by means of chemical solution deposition has already been reported elsewhere [1]. A fine tuning of nanodots’ size, morphology and density has been achieved through the control and modification of precursor solution concentration and growth conditions (temperature, time and atmosphere). Here we apply this methodology to BaZrO3 (BZO). The interest of this study is twofold: first, from the fundamental point of view, it offers a new scenario for the investigation of self-assembling phenomena of oxide nanodots grown from chemical solutions and secondly, because such nanostructured surfaces can be used as templates for the growth of optimized YBCO films. In this work, the microstructure of self-assembled BZO nanoislands generated following a very general bottom-up approach, based on the deposition of chemical solutions, has been investigated using cross-section transmission electron microscopy. TFA-derived YBCO has been deposited on the nanostructured template and the effects of the nanodots on the YBCO lattice has been studied. Two samples have been investigated: one deposited from 0.03M solutions and annealed at 900ºC for 4h in O2, and the other one deposited from a 0.003M solution. On one hand, low magnification TEM images of the 0.03M sample reveal a pronounced bimodal size distribution of particles. Larger particles have dimensions within the range 300 to 400nm and outcrop from within a nanocrystalline film homogeneously covering the substrate. A higher magnification image of the nanocrystalline fraction of the film shows that it is composed by nanocrystals of a tetragonal Ba-Zr oxide phase. Selected area electron diffraction patterns featured very weak diffraction rings consistent with a completely random orientation of this nanocrystalline fraction of the film. On the other hand, for the most diluted precursor solution (0.003M), there is an evolution of the system from the polycrystalline, randomly oriented microstructure to well-separated cube on cube epitaxial cubic BZO nanodots. In this case, BZO grown on LAO and STO substrates present a narrow size distribution of 10 - 20 nm in weight and 5 - 10 nm in height, which has been determined by AFM and confirmed by TEM. Furthermore, AFM analysis reveals BZO nanodots are basically localized close to step edges. HRTEM analysis reveals that BZO forms a self assemblage of well separated cube-on-cube epitaxial islands and are commonly facetted {100} and {110} planes, Figure 1.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 291–292, DOI: 10.1007/978-3-540-85226-1_146, © Springer-Verlag Berlin Heidelberg 2008
292
(a)
(001) (01-1)
(010) (01-1)
(b)
(010) (011)
Figure 1. (a) High resolution TEM image of a BZO nanodot grown on LAO single crystal from a solution having a concentration of 0.003M; the nanodots are mainly faceted {100} and {110} planes. (b) AFM image showing a narrow size distribution of the self-assembled nanodots. Observation of strain fields associated with interfacial defects indicates that the BZO nanodots are fully relaxed.
Figure 2. High resolution TEM image of a BZO nanodot at the interface between the YBCO film and the LAO substrate. A high resolution TEM image of an interfacial BZO nanodot, corresponding to a template where YBCO has been deposited, is shown in Figure 2. The image clearly reveals strong bending of the (001) planes at the interface with the nanodot, demonstrating that the presence of the nanodots may disturb the YBCO lattice, while no threading dislocations originating from the nanodots have been identified yet. Epitaxial YBCO quality is preserved in the presence of interfacial BZO dots but, however, in standard growth conditions, the presence of interfacial nanodots enhances the nucleation of a-oriented domains. 1. 2.
M. Gibert, T. Puig and X. Obradors, Surf. Sci. 601 (2007), 2680 This work has been supported by EU (HIPERCHEM project), Generalitat de Catalunya (2005-SGR-0029 and CeRMAE) and by Spanish MEC (MAT2005-02047, FPU program)
293
Hydrothermal synthesis and characterisation of single crystal α-Fe2O3 nanorods T. Almeida, Y.Q. Zhu and P.D. Brown School of Mechanical, Materials and Manufacturing Engineering, The University of Nottingham, University Park, Nottingham, NG7 2RD, United Kingdom [email protected] Keywords: hydrothermal synthesis, α-Fe2O3, β-FeOOH, nanorod
One-dimensional (1D) nanostructures have attracted extensive attention due to their novel magnetic properties which are greatly dependent on nanorod size and shape [1]. If the particle size decreases toward a critical value it can consist of a single magnetic domain. Further, a 1D magnetic nanostructure can exhibit much higher coercivity than its isotropic counterpart because of the effect of shape anisotropy. Ferromagnetic hematite (α-Fe2O3) is of particular interest because of its low cost, high resistance to corrosion and environmentally friendly properties. Hydrothermal synthesis (HS) is a comparatively simple process for the preparation of 1D iron oxide nanostructures. However, the mechanism of nanorod formation is not clearly understood, thereby preventing the effective control of α-Fe2O3 nanorod size, shape and growth. α-Fe2O3 nanorods offer many opportunities with applications in fields such as drug delivery, gas sensors and magnetic data storage. A systematic experimental programme has been undertaken to investigate the effect hydrothermal processing conditions on the controlled production of 1D α-Fe2O3 nanostructures. At low hydrothermal temperatures, small β-FeOOH nanorods nucleate from an initial aqueous FeCl3 solution, as shown in Figure 1a. With increasing hydrothermal temperature, an enhancement in the atomic vibration of β-FeOOH molecules results in the breaking of hydrogen bonds, and through the loss of OH- ions [2], the nanorods agglomerate and transform into larger, more thermally stable α-Fe2O3 nanoparticles. The aspect ratio of the nanoparticles may be controlled by the addition of a phosphate surfactant [3]. The PO43- anions have a marked effect on the manner in which small β-FeOOH nanorods align before crystallisation (Figure 1b). The surfactant, however, restricts the dehydration of β-FeOOH and hence suppresses phase transformation into α-Fe2O3. Thus, at higher PO43- concentrations, higher reaction temperatures are required to produce single crystal lenticular α-Fe2O3 nanorods with high aspect ratio (Figure 2). A thorough exploration of the HS growth conditions has been performed using the combined complementary characterisation techniques of transmission electron microscopy (TEM), selected area electron diffraction (SAED), Fourier transform infra-red (FTIR) spectrometry, X-ray diffractometry (XRD) and Xray photoelectron spectrometry (XPS). Through clear understanding of the growth mechanism, it becomes possible to control the size and shape of these 1D α-Fe2O3 nanorods. The importance is made clear
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 293–294, DOI: 10.1007/978-3-540-85226-1_147, © Springer-Verlag Berlin Heidelberg 2008
294
when α-Fe2O3 becomes super-paramagnetic below certain dimensional values, making it ideal for contrast media applications, e.g. in magnetic resonance imaging [4].
Figure 1. TEM micrographs showing (a) small β-FeOOH nanorods produced through HS at 120˚C and (b) the alignment of β-FeOOH nanorods through the addition of a phosphate surfactant.
Figure 2. A single crystal lenticular α-Fe2O3 nanorod produced through HS at 200˚C. 1. 2. 3. 4.
G.Bate, J. Magn, Magn. Mater. Vol 100 (1991) 413 Y. Sui, D. Xu and W.Su, Materials Research Bulletin, Vol 30, No 12 (1995) 1553-1560 T. Sugimoto, Y. Wang, H. Itoh and A. Muramatsu, Colloids Surf. A Vol 134 (1998) 265 Lawaczeck.R, Menzel.M, Pietsch.H, Applied Organometallic Chemistry, Vol 18 (2004) 506
295
GaAs NWs and Related Quantum Heterostructures Grown by Ga-Assisted Molecular Beam Epitaxy: Structural and Analytical Characterization J. Arbiol1,2, S. Estradé2, F. Peiró2, J.R. Morante2, C. Colombo3, D. Spirkoska3, G. Abstreiter3 and A. Fontcuberta i Morral3 1. TEM-MAT, Serveis Cientificotècnics, Universitat de Barcelona, E-08080 Barcelona, CAT, Spain 2. EME/CeRMAE/IN2UB, Departament d’Electrònica, Universitat de Barcelona, C/ Martí i Franquès 1, E-08080 Barcelona, CAT, Spain 3. Walter Schottky Institut, Technische Universität München, D-85748 Garching, Germany [email protected] Keywords: GaAs NWs, MBE, heterostructure, TEM, HAADF, EELS.
Molecular Beam Epitaxy has been for the last two decades the most established technique for the realization of atomically precise nanostructures such as quantum wells, wires and dots. To date the epitaxial precision has been limited to the plane of growth. On the other hand, semiconductor nanowires constitute promising building blocks for next generations of electronic and optoelectronic devices. The use of Molecular Beam Epitaxy (MBE) for the synthesis of ultra-pure 1-D nanostructures has been recently demonstrated. In particular, GaAs nanowires along the [111] direction have been grown avoiding the use of Au as nucleation seeds [1]. The use of the MBE allows us to control the growth conditions during the synthesis and thus being able to tune from 1D to 2D deposition. This latter option led us obtain high quality coaxial GaAs/AlGaAs quantum heterostructures with a perfect epitaxy between the different material layers [2]. In the present work, we will show the structural, morphological and elemental characterization of ultra-pure GaAs NWs and GaAs/AlGaAs coaxial quantum heterostructures grown by molecular beam epitaxy avoiding catalytic seeds. In order to perform the high detail characterization at atomic scale we will use high resolution transmission electron microscopy (HRTEM) and scanning transmission electron microscopy (STEM) in bright field and Z-contrast modes. Electron energy loss spectroscopy will be used to obtain the compositional profiles and maps, which will allow us to distinguish the sharpness in composition of the quantum heterostructures. Special emphasis will be focused on the epitaxial relationships between the different layers of the quantum heterostructures and also on the orientation of the nanowires versus the substrate [2]. The possible crystalline defects will be analyzed (such as lamellar twinning [3,4,5,6]) and the effects of the substrate orientation (Si [001] or [111]) on the nanowire growth and homogeneity of the designed quantum wells commented.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 295–296, DOI: 10.1007/978-3-540-85226-1_148, © Springer-Verlag Berlin Heidelberg 2008
296
1. 2. 3. 4. 5. 6.
A.F.I. Morral, C. Colombo, G. Abstreiter, J. Arbiol, J. R. Morante, Applied Physics Letters, 92 (2008), 063112. A.F.I. Morral, D. Spirkoska, J. Arbiol, J. R. Morante and G. Abstreiter, Small, (2008) in press. J. Arbiol, B. Kalache, P. Roca i Cabarrocas, J. R. Morante, A.F.I. Morral, Nanotechnology, 18 (2007), 305606. J. Arbiol, A.F.I. Morral, S. Estradé, F. Peiró, B. Kalache, P. Roca i Cabarrocas, J. R. Morante, Nanotechnology, (2008) in press. F.M. Davidson, D.C. Lee, D.D. Fanfair, B.A. Korgel, J. Phys. Chem. C 111 (2007), 29292935. L.S. Karlsson, K.A. Dick, J.B. Wagner, J.O. Malm, K. Deppert, L. Samuelson, L.R. Wallenberg, Nanotechnology, 18 (2007), 485717.
BFSTEM
Z-STEM
GaAs Core
GaAs Core
AlAs AlAs GaAs QW
GaAs QW
AlAs AlAs
Z-STEM
GaAs Core
2.0 nm1.8 nm2.0 nm AlAs GaAs AlAs QW
Figure 1. BF-STEM and HAADF Z-contrast STEM analysis of a coaxial GaAs/AlAs quantum well heterostructure, viewed along the NW growth axis.
297
A method for in-situ electrical measurements of thin film heterostructures using TEM and SEM J. Börjesson1, A. Kalabukhov2, K. Svensson1 and E. Olsson1 1. Microscopy and Microanalysis, Chalmers University of Technology, SE-41296 Göteborg, Sweden 2. Microtechnology and Nanosience, Chalmers University of Technology, SE-41296 Göteborg, Sweden [email protected] Keywords: In-situ TEM, In-situ SEM, STM
A method for in-situ measurements of electrical properties of thin film heterostructures using TEM and SEM has been developed. This method allows measurements of the conductance in a thin film heterostructure in a direction along the film planes in thin TEM foils. The advantage is that the properties can be directly correlated to the local atomic structure. The specimens are cross section TEM samples prepared with standard grinding, polishing and ion beam milling techniques. The equipment used for the measurements is a scanning tunnelling microscope (STM) that can be inserted in both a TEM holder and on a SEM stage. The spatial precision of the STM tip motion is on the atomic scale [1]. The STM tip can translated be controlled in x-, y- and z-direction with both a coarse and a fine motion mode. Figure 1 shows a schematic of a typical TEM thin film cross-sectional sample and the instrument setup. A combined focused ion beam (FIB) workstation and a scanning electron microscope (SEM) is used to create a micrometer sized back contact from the specimen to the 3mm TEM aperture. A tailored screening method is used to protect the electron transparent region of the specimen from ion beam radiation in the FIB/SEM instrument. The advantage to first performing the measurements in a SEM is that it offers a larger field of view and additional information about the three dimensional geometry of the sample and the STM tip. It also makes it possible carry out reference measurements on parts of the sample that is not electron transparent. The measurements performed in-situ in a TEM enable higher spatial precision in the positioning STM tip with respect to the sample. This makes it possible to measure the electrical properties of thin film layers and heterostructures (see Figure 2) and also study the influence of interfaces and local defects. The TEM provides additional information about the specimen microstructure. In addition to the information extracted from the SEM. 1. 2.
K. Svensson, Y. Jompol, H. Olin and E. Olsson, Review of Scientific Instruments 74 (2003), p. 4945. Support from Nanofactory Instruments is gratefully acknowledged for technical support.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 297–298, DOI: 10.1007/978-3-540-85226-1_149, © Springer-Verlag Berlin Heidelberg 2008
298
Figure 1. Schematic of (a) a standard TEM thin film cross-sectional sample with a Platinum back contact made by FIB/SEM and (b) the experimental setup with the TEM sample and the STM tip. Electrical measurements are possible by controlling the voltage and measuring the current between tip and sample as a function of position on the specimen.
Figure 2. A TEM micrograph of a thin film superlattice of La1-xSrxMnO3 (blue), LaAlO3 (green) and SrTiO3 (yellow) on an NbGaO3 substrate (red). Courtesy to Boschker, University of Twente, for supplying the thin film heterostructure.
299
Electron Beam Nanofabrication and Characterization of Iron Compounds K. Furuya1, M. Shimojo1,2, M. Takeguchi1, M. Song1, K. Mitsuishi1 and M. Tanaka1 1. National Institute for Materials Science; 3-13 Sakura; Tsukuba, 305-0003 JAPAN 2. Advanced Science Research Laboratory; Saitama Institute of Technology; 1690 Fusaji; Fukaya, Saitama, 369-0293, JAPAN [email protected] Keywords: electron beam nanofabrication, iron antenna, iron oxide nanostructures
The production of nanometer-sized oxide structures is of significant interest due to the potential application to nanoelectronics, nanomagnetics and optoelectronics. It is important to place nano-dots or nano-wires at desired positions for the production of nanodevices. Electron beam-induced deposition (EBID) is a promising technique to produce such dots and wires [1]. The resolution of EBID is now reaching down to subnanometers [2]. Recently, Shimojo et al. reported that carbon-free crystalline iron oxide was deposited at room temperature by EBID [3]. In this paper, effects of water and oxygen addition to iron pentacarbonyl on nanostructure are studied. EBID was carried out in a 30kV FE-SEM (JSM-7800UHV) with a custom made gas introduction system. A schematic illustration of the deposition system is shown in Figure 1 [3]. The electron beam current was 0.8 nA with a beam diameter of 4 nm. The base pressure of the chamber was 2x10-6 Pa. Two cylinders, either 1) iron pentacarbonyl (Fe(CO)5) and water (H2O) or 2) Fe(CO)5 and oxygen (O2) were connected. The electron beam position was controlled by an external deflection with a PC. A high resolution TEM image and a diffraction pattern of nanorods formed using a mixture of Fe(CO)5 and H2O vapors are shown in Figs. 2(a) and 2(b). The partial pressure ratio [H2O]/[Fe(CO)5] was 1.0. Crystalline Fe3O4 iron oxide was seen to be formed, by analyzing the diffraction pattern. No amorphous carbon is observed in the nanorods. It is suggested that oxygen radicals formed from water molecules remove carbon and oxidize iron. The composition of the deposits as a function of partial pressure ratio, [H2O]/[Fe(CO)5] is shown in Figure 2(c). The carbon content decreased with increasing the partial pressure ratio, and reached almost zero at partial pressure ratio of 1.0 or more. The ratio of Fe and O became constant at partial pressure ratio of more than 1.0. Figure 3 shows a high resolution TEM image of a nanorod formed with Fe(CO)5 mixed with O2 at a partial pressure ratio [O2]/[Fe(CO)5] of 1.0. Fast Fourier transforms of parts of the high resolution image near the surface and inside regions are also shown. Both reveal that small crystals exist near the surface but the inside is amorphous. The mechanism will be discussed in the talk. 1.
M. Shimojo, K. Mitsuishi, A. Tameike and K. Furuya: J. Vac. Sci. Technol. B 22 (2004) 742.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 299–300, DOI: 10.1007/978-3-540-85226-1_150, © Springer-Verlag Berlin Heidelberg 2008
300
2. 3.
W. F. van Dorp, B. van Somern, C. W. Hagen and P. Kruit: Nano Lett. 5 (2005) 1303. M. Shimojo, M. Takeguchi and K. Furuya: Nanotechnology, 17 (2006) 3637.
Figure 1. Schematic drawing of a 30 kV FESEM with dual gas introduction system for EBID with a gas of iron carbonyl
Figure 3. High resolution TEM image (a) of a nanorod formed with Fe(CO)5 mixed with O2 at a partial pressure ratio [O2]/[Fe(CO)5] of 1.0. Fast Fourier transforms of parts of the high resolution image near the surface (b) and inside (c) regions.
Figure 2. High resolution TEM image (a) and a diffraction pattern (b) of nanorods formed at a partial pressure ratio of 1.0, and the composition of the deposits as a function of partial pressure ratio (c), using a mixture of Fe(CO)5 and H2O.
301
TEM analysis of the chemical gradient in (Zn,Mn)Te/ZnTe nanowires H. Kirmse1, W. Neumann1, S. Kret2, P. Dłużewski2, E. Janik2, W. Zaleszczyk2, A. Presz3, G. Karczewski2, T. Wojtowicz2 1. Humboldt-Universität zu Berlin, Institut für Physik, AG Kristallographie, Newtonstraße 15, D-12489 Berlin, Germany 2. Institute of Physics, PAS, Al. Lotników 32/46, 02-668 Warsaw, Poland 3. Institute of High Pressure Physics, PAS, Sokołowska 29/37, 01-142 Warsaw, Poland holm kirmse@physik hu-berlin.de Keywords: (Zn,Mn)Te, nanowires, analytical TEM
Magnetic semiconductor nanowires (NWs) are subject of intense fundamental research due to their potential applicability in the field of spin-based electronics. In general, NWs are several micrometers long and only a few tens of nanometers in diameter. Our previous work focussed on the understanding of the structural and chemical properties of ZnTe NWs [1-3]. These NWs were grown on GaAs substrates via a vapour-liquid-solid (VLS) growth regime using a Au-based catalyst droplet. The growth of current (Zn,Mn)Te diluted magnetic semiconductor NW structures was based on the same VLS mechanism and performed at 380 °C in a molecular beam epitaxy machine. The orientation of the GaAs substrate was (110). As seen in the SEM images of Figure 1 the length of the (Zn,Mn)Te NWs amounts to about 400 nm after a period of 15 min (Figure 1a). The combination of 15 min (Zn,Mn)Te and 15 min ZnTe growth reveals an overall length of the NWs of about 1.5 µm. Hence, the growth rate of ZnTe part is twice as large than the apparent growth rate of the (Zn, Mn)Te pedestal. In order to analyse the sharpness of the (Zn,Mn)Te/ZnTe interface, analytical TEM was applied. For localizing the interface a series of EDX point spectra was acquired along the NW axis (cf. Figure 2). Comparing the Mn-K signals of positions 2 and 3 (Figure 2b) a decrease is found due to the termination of the Mn molecular beam after 15 min. The interface is located at a position of about 400 nm. The slow exponential decrease of the Mn signal for the positions 3 to 6 hints either to a high content of Mn still present in the catalyst droplet after closing the Mn shutter or to a strong Mn interdiffusion. The decreasing background signal is due to the shape of the NW. Observing the bottommost area around the NWs a compact layer is seen. Zn, Mn and Te are detected in this area. Moreover, Au and Ga, forming the eutectic catalyst present at the tip of each NW, is found in the layer. In agreement to the results for the NWs a decrease of the Mn content is detected from position A to B whereas Zn increases (see Figure 3b). In the visualized area the layer is separated from the GaAs substrate (cf. Fig. 3a), although in general, this layer is in contact with the substrate. Due to the epitaxial relation between NWs and the substrate, the NWs grow along the two 〈111〉 directions sticking out of (110)-oriented GaAs substrate, as visible in all figures.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 301–302, DOI: 10.1007/978-3-540-85226-1_151, © Springer-Verlag Berlin Heidelberg 2008
302
1. 2. 3. 4.
E. Janik, J. Sadowski, P. Dluzewski, S. Kret, L.T. Baczewski, A. Petroutchik, E. Lusakowska, J. Wróbel, W. Zaleszczyk, G. Karczewski, and T. Wojtowicz, Appl. Phys. Lett.89 (2006) p. 133114. E. Janik, P. Dluzewski, S. Kret, A. Presz, H. Kirmse, W. Neumann, W. Zaleszczyk, L.T. Baczewski, A. Petroutchik, E. Dynowska, J. Sadowski, W. Caliebe, W. Wojtowicz Nanotechnology 18 (2007) p. 475606. H. Kirmse, W. Neumann, S. Kret, P. Dłużewski, E. Janik, G. Karczewski, T. Wojtowicz, IOP Conf. Series, Proc. 15th Conf. on Microscopy of Semiconducting Materials, April, 2nd to April 5th, 2007, Cambridge, United Kingdom, in print The research was partially supported by the Ministry of Science and Higher Education (Poland) through grants N507 030 31/0735, N515 015 32/0997 and by the Network "New materials and sensors for optoelectronics, information technology, energetic applications and medicine", and by the Foundation for Polish Science through subsidy 12/2007.
Figure 1. SEM images of growth states of (Zn,Mn)Te/ZnTe NWs; left: 15 min growth of (Zn,Mn)Te (after 15 min the main shutter was introduced in front of this substrate), right: 15 min growth of (Zn,Mn)Te and 15 min growth of ZnTe, respectively.
200 nm
Figure 2. Composition analysis of a (Zn,Mn)Te/ZnTe NWR; left: HAADF STEM image, right: EDX intensity of the Mn-K line for the positions given in the image on the left.
Figure 3. Formation of a layer; left: HAADF STEM image with marker of the EDX line scan given on the right.
303
Structural and morphological characterization of GaN/AlGaN quantum dots by transmission electron microscopy M. Korytov1, M. Benaissa2, J. Brault1, T. Huault1 and P. Vennéguès1 1. CRHEA-CNRS, Rue Bernard Grégory, Sophia Antipolis, 06560 Valbonne, France 2. CNRST, 52 Bd Omar Ibn Khattab, BP 8027, Agdal, 10102 Rabat, Morocco [email protected] fr Keywords: HRTEM, HAADF, quantum dots, MBE
In recent years much attention has been devoted to GaN quantum dots (QDs) due to their potential application as light emitting diodes and lasers diodes operating in the ultra-violet range. QDs allow carriers localisation thus diminishing the influence of the dislocations existing in III-nitrides films on light emission efficiency. The majority of GaN QDs are grown on AlN templates. In this study structural and morphological characterization of GaN QDs grown on Al0 5Ga0 5N templates was carried out by transmission electron microscopy. The main advantage of AlGaN alloys over pure AlN substrate is a possibility to be doped, which enables using GaN QDs as a base for light-emitting devices. The samples under investigation were grown by molecular beam epitaxy using ammonia as nitrogen source and they were composed of three buried layers and one surface layer of GaN QDs separated by AlGaN spacers [1]. A series of samples with varying GaN nominal thicknesses was made. All specimens were studied by High-Resolution Transmission Electronic Microscopy (HRTEM) and High Angular Annular Dark Field (HAADF) technique. HRTEM images were taken under (0004) two-beam conditions. For that the sample was tilted about 6º degree out of the [1120]-zone axis along the [1100] direction to minimize number of the incidental beams. The (0002) beam was centred on the optic axis and the images were formed by using only direct (0000) and one reflected (0002) beams to diminish influence of the change of the local sample thickness and the objective lens defocus to HRTEM contrast [2]. Lost of resolution in the (0002) plane does not hamper the analysis since only distances between basal planes need to be measured. HRTEM images were treated by the Geometrical Phase Analysis (GPA) method, which visualize increase of the local lattice parameter (LLP) into GaN QDs against Al0 5Ga0 5N spacers (Figure 1). HAADF technique was used to obtain chemical contrast in the QDs region (Figure 2). Two main results have to be reported. Firstly, above a critical thickness of deposited GaN, we observed a morphological transition between surface QDs which have a pyramidal shape and buried ones which have a truncated pyramid shape as typically reported for GaN/AlN QDs. Secondly, a stress-driven phase separation in the AlGaN spacers with the formation of Al-rich zones above the QD and Ga-rich zone between QDs was found. Such behaviour with alternating Al- and Ga-rich regions may allow a
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 303–304, DOI: 10.1007/978-3-540-85226-1_152, © Springer-Verlag Berlin Heidelberg 2008
304
spatial correlation of QDs between successive QDs layers for sufficiently thin AlGaN spacers. 1. 2.
T. Hualt, J. Brault, F. Natali, B. Damilano, D. Lefebvre, L. Nguyen, M. Leroux and J. Massies, APL 92, 051911 (2008) D. Gerthsen, E. Hahn, B. Neubauer, V. Potin, A. Rosenauer, and M. Schowalter, Phys. Stat. Sol (c) 0, No. 6, p. 1668-1683 (2003)
Figure 1. A) HRTEM image of single QD and B) LLP colour-coded map obtained by GPA treatment of the previous image.
Figure 2. HAADF image of two QDs. More bright regions correspond to heavier elements.
305
Structure and stability of core-shell AuAg nanopartciels Z.Y. Li1, R. Merrifield1, Y. Feng1, J.P. Wilcoxon1, R.E. Palmer1, A.L. Bleloch2, M. Gass2 and K. Sader2 1. Nanoscale Physics Research Laboratory, School of Physics and Astronomy, University of Birmingham, Birmingham B15 2TT, U.K. 2. SuperSTEM Laboratory, STFC Daresbury, Daresbury WA4 4AD, U.K. [email protected] Keywords: STEM, absorption, core-shell nanoparticles
Nanopartciels comprising two different metallic elements offer additional degrees of freedom for altering their physical properties by varying the atomic composition and atomic arrangement. This could potentially enable a wide range of applications for discovering materials with novel physical properties. However, our present understanding of fundamental issues has been hindered by the lack of knowledge of the precise chemical composition and atomic arrangement within a given bimetallic nanoparticle. Here, we report our recent systematic study on structural and optical properties of core/shell structured AgAu nanoparticles of 4-5 nm diameter by a combination of high resolution scanning transmission electron microscopy (STEM) with UV-visible absorption spectroscopy. The nanoparticles were synthesised by first growing a seed nanocrystal (either Ag or Au) followed by solution phase deposition of several generations of overlayers of shell materials (Au or Ag). The particles were passivated with C12SH during the growth process [1]. Figure 1 shows a comparison of absorption spectra taken from toluene solutions containing core/shell AgAu nanoparticles, revealing strong plasmon resonances and discernable differences in plasmon frequency with different growth sequences. However, optical measurements provide average information that may or may not reflect the heterogeneous nature of bimetallic nanoparticles. Therefore, it is extremely important to develop methods having a high spatially-resolved imaging capability for the internal structure to correlate nanostructure with optical properties. Characterising the core-shell structure of AgAu nanoparticles is a challenging task, as both elements have almost identical lattice spacing. We show that, by utilising the large difference in the atomic numbers of Ag (Z=47) and Au (Z=79), high-angle annular dark field (HAADF) imaging using STEM is capable of determining the possible composition modulation within the nanoparticles [2]. The insert in Figure 1 displays typical three-dimensional plots of Z-contrast images (taken by aberration-uncorrected Tecnai F20 STEM) from the corresponding core/shell AgAu particles. Although no atomic lattice is resolved, distinctly different HAADF intensity contrast variation in two core/shell nanoparticle systems is apparent. It is worth of noting that in the present case, the shell thickness is only 1-2 atomic layers, demonstrating the impressive sensitivity of HAADF-STEM based Z-contrast imaging technique. Using the current generation aberration-corrected STEM, one can obtain further details of internal
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 305–306, DOI: 10.1007/978-3-540-85226-1_153, © Springer-Verlag Berlin Heidelberg 2008
306
structural and chemical information at atomic-scale. Figure 2 displays one of such examples, where atomic arrangement is clear within Ag core/Au shell nanoparticles. To understand the structure of core/shell AgAu nanoparticles, we consider factors controlling the thermodynamics stability of nanoparticles, including surface energy, cohesive energy and strain, etc. All these factors favour for Ag being at the surface or to form alloyed interface with Au. Our study show that ‘inverted’ Ag/Au nanoparticles can be synthesised suggesting that this structure is at least kinetically stable, though the role that the passivated ligands play needs to be taken into account. In summary, we have successfully demonstrated that the HAADF-STEM imaging is a powerful technique to study the internal structures of core-shell nanoparticles and their evolution. This opens up unprecedented opportunities for detailed investigation on structure/property relationship of these individual building blocks of potential novel functional materials 1. 2.
Z.Y. Li, J.P. Wilcoxon, F. Yin, Y. Chen, R.E. Palmer, R.L. Johnston, Faraday Discussion, 138 (2008) 363-373. Z.Y. Li, J. Yuan, Y. Chen, J.P. Wilcoxon, R.E. Palmer, Appl. Phys. Lett. 87 (2005) 243103.
Figure 1. Three-dimensional HAADF intensity profiles of single AgAu core-shell nanoparticles with UV-visible absorption spectra obtained from the solution containing corresponding nanoparticles. The atomic composition of Ag and Au is 1:1.
a
b Figure 2. Unprocessed (a) and filtered (b) HAADF images of a Ag(core)/Au(shell) nanoparticle by aberration-corrected STEM at SuperSTEM facility.
307
In-situ studies on electrical and mass transport in multi-wall carbon and vanadium oxide nanotubes M. Löffler, T. Gemming, R. Klingeler, B. Büchner IFW Dresden, P.O. Box 270116, 01171 Dresden [email protected] Keywords: nanotubes, in-situ, STM
The determination of electronic and mechanical properties of nanoscale materials often presents a challenge with regards to handling and contacting individual structures rather than measuring bulk-scale average properties. In our setup, an in-situ scanning tunneling microscope (STM) is used inside a transmission electron microscope (TEM) to study the influence of electric fields and biases on these individual nanostructures while at the same time observing mechanical and/or structural changes. Electrical and concomitant mass transport in iron filled multi-wall carbon nanotubes (MWCNT) driven by electromigration has been studied (Figure 1). The necessary switching current densities, reversibility and respective breakdown current densities of the empty MWCNT using biases in the range of 0-10V have been measured (c f. [1]). Furthermore, deflections of the nanotubes by a Lorentz-force under current flow have been observed (Figure 2). Contact resistances, which are of great influence in 2-point measurement setups, have been reduced by pulsed, current-driven annealing. The same setup has been used to determine resistances of individual vanadium-oxide nanotubes (VOxNT) and respective I-V-curves with good reproducibility. For the first time, ohmic characteristics with electrical resistances down to 40MΩ have been observed on VOxNT (cf. [2]) between two tungsten STM-tips as well as in tube-tube junctions between VOxNT (Figure 3). This work presents a starting point for measuring important electronic and electromechanical properties of filled and/or doped carbon and oxide-based nanoscale materials [3]. 1. 2. 3.
K. Svensson, E. Olin, E. Olsson, Phys. Rev. Lett. 93 (2004), 145901 L. Krusin-Elbaum, D. M. Newns, H. Zeng, V. Derycke, J. Z. Sun, R. Sandstrom, Nature 431 (2004), 672-676 This work is funded by the „Pakt für Forschung“ We want to thank U. Weissker, I. Hellmann for the samples and S. Leger for technical assistance.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 307–308, DOI: 10.1007/978-3-540-85226-1_154, © Springer-Verlag Berlin Heidelberg 2008
308
+3.6V
-3.6V
Figure 1. Electromigrative movement of the iron filling inside a double-wall CNT. The switching current density is in the order of 10GA/cm2
Voltage Figure 2. Double image of one and the same MWCNT produced by vibration. The cause for vibration is the change of the Lorentz-force due to an AC-current and the static magnetic field of the objective lens. At high currents (top) the filling clearly extends and is assumed to be in the molten state.
Figure 3. Left: Vanadium-oxide nanotube between two tungsten STM-tips. Right: Junction between two VOxNT of different diameter.
309
Electron microscopy of nano-magnesium produced by Inert Gas Condensation for hydrogen storage E. Piscopiello1*, E. Bonetti2, E. Callini2, L. Pasquini2 and M. Vittori Antisari1 1. FIM Department, ENEA, C.R. Casaccia C.P. 2400, 00123 Rome, Italy. * C.R. Brindisi, via Appia km 706, Brindisi, 72100, Italy. 2. Department of Physics, Università di Bologna and CNISM, viale Berti Pichat 6/2, 40127 Bologna, Italy. [email protected] Keywords: Inert Gas Condensation, Magnesium, hydrogen storage.
Several issues have been extensively explored in last years in order to improve the hydrogen sorption properties of magnesium for Hydrogen storage. Among other parameters, the material microstructure and particle size play an important role, even if a detailed description of the elementary processes behind the reaction of Mg with gaseous hydrogen are still far to be completely understood [1]. In order to prepare model system having a well defined structure, the Inert Gas Condensation (IGC) technique is extremely powerful, since it allows the formation of dispersed nanoparticles or clusters even with a core shell structure. TEM investigations have been used to study the morphological and structural properties of ICG Mg particles obtained by varying the He gas pressure (0.02÷2 mbar) in the condensation chamber. To this purpose, a FEI Tecnai G2 30F microscope, equipped with a Schottky field emission source and operating at 300kV has been used. Experimental results show that the gas pressure in the IGC chamber affects both the average particle size and the perfection of the structure, as it can be seen in the images reported in Figure 1 (a, b, c). In all batches, the Mg crystals display often a six-fold symmetry which can be correlated with the hexagonal structure of Mg, so that most of the sample is made of (0001) oriented particles as confirmed by the high resolution image reported in Figure 1 (c). Moreover the lateral surface of the particle appears to be decorated with an oxide layer, while the (0001) surface appears to be relatively free from oxygen. The sample produced at the lowest He pressure (0.02mbar, Figure 1(a)) appears to have the smallest average particles size, of the order of a few tens of nm, and a narrower distribution function, while particles synthesized at higher He pressures are larger by about one order of magnitude and with a broad size distribution. High resolution observations showed that in the latter case the particles are single crystal with a perfect structure while in the former a mosaic structure can be observed. The morphological and structural properties of the particles affect the hydrogen sorption behaviour. In fact the particles synthesized at lower pressure show a lower hydrogen desorption temperature (Figure 1(d)) indicating that crystal defects and particle size assists the phase transformation and the hydrogen transport at the free surface.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 309–310, DOI: 10.1007/978-3-540-85226-1_155, © Springer-Verlag Berlin Heidelberg 2008
310
In conclusion, the He pressure in the IGC synthesis chamber strongly affects the Mg particle structure with evident effects on the kinetics of reaction with hydrogen. TEM analyses allow an interpretation of the sorption properties on the base of particle microstructure. 1.
A. Zuttel, Materials for Hydrogen Storage, Mater . Today, 6 (2003), pp. 24-33.
(b)
(a)
100nm
(c)
Mg 0,02 mbar
Mg 2 mbar He
200nm
(d)
5nm Figure 1. TEM images of the Mg nanocrystals prepared by IGC at different He pressure, as indicated: 0.02mbar (a) and 2 bar (b). (c) HRTEM image of the border of one particle from the sample synthesized at 2mbar. It is possible to notice the lateral oxide layer and the hexagonal symmetry of the lattice, coherent with the particle shape. Figure 1(d) reports the MgH2 DSC runs, Ar atmosphere, 10 K/min, obtained from particles synthesized at 0.02 and 2mbar of He pressure.
311
Two Different Structures of Crystalline Mesoporous Indium Oxide Obtained by Nanocasting Process E. Rossinyol1, E. Pellicer2,3, M. Cabo3, O. Castell1 and M.D. Baro3 1. Microscopy Services, Faculty of Science, Universitat Autonoma de Barcelona, 08193 Bellaterra, Barcelona, Spain. 2. Institut Catala de Nanotecnologia, Campus de la Universitat Autonoma de Barcelona, Edifici Q (ETSE), 08193 Bellaterra, Barcelona, Spain. 3. Departament de Física, Edifici Cc, Universitat Autonoma de Barcelona, ES-08193 Bellaterra, Barcelona, Spain. [email protected] Keywords: mesoporous, indium oxide, nanocasting
Crystalline mesoporous metal oxides with narrow pore size distributions and controllable morphologies are interesting in a wide range of applications such as gas sensing, optics or catalysis. The synthesis pathway known as nanocasting is based in the growth of metal and semi-conductor nanoparticles within the pores of a regular mesoporous material. The use of the regular channels of ordered mesoporous silica as matrices for the controlled growth of nanoparticles and nanorods has been widely reported. In this method, the three-dimensional pore system of the matrix is filled with a suitable metal oxide precursor, which is then converted to the oxide during the calcination process. The structure matrix is finally removed, yielding the metal oxide as its negative replica. This nanocasting method has allowed the synthesis of numerous mesoporous metal oxides, many of which were formerly unavailable by the conventional synthesis method of supramolecular structure direction. Indium is a low melting point metal, which can easily be oxidised into indium oxide (In2O3). Indium oxide is a transparent n-type semiconducting oxide with a band gap of around 3.6 eV, which is known to exhibit luminescence1 and gas sensing2 properties. In addition, indium oxide nanofibers3 and nanosized particles dispersed within pores of non-organised mesoporous silica4 have been reported to give photoluminescent properties. For our aim, two different mesoporous silica structures were chosen: i) the 3D cubic (space group Ia3d) named KIT-6, which is probably the most complex one presenting a double gyroidal mesostructure with channels running along the [100] and [111] directions, defining a 3D pore network;4 ii) the 2D hexagonal structure (space group p6mm) named SBA-15, which has a simpler structure. Both templates have been used for the synthesis of mesoporous indium oxide nanostructures that were compared and have shown evidence of possible structure effects on the electronic properties. Different catalytic additives have been introduced and their effect have been analysed. In2O3 powder was synthesized by impregnation of 0.15 g mesoporous SBA-15 and KIT-6 silica template with 0.39 g In(NO3)3 · xH2O (purchased from Aldrich) in ethanol. Fully details of silica template synthesis were reported elsewhere6. After the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 311–312, DOI: 10.1007/978-3-540-85226-1_156, © Springer-Verlag Berlin Heidelberg 2008
312
impregnation step, the resulting mixtures were dried and calcined at 350 °C for 4 h. Then, a second impregnation was carried out by mixing the powder obtained with 0.22 g of indium nitrate precursor. After 30 min of stirring, samples were dried and calcined again at 600 °C for 4 h. Finally, the silica template was removed with NaOH solution. The slurry obtained was centrifuged, copiously washed and dried. Catalytic additives were added by impregnation. Water used had been distilled twice and deionized with a Millipore Milli Q system. In the wide-angle XRD patterns of the In2O3 powders, the main diffraction peaks correspond to cubic Ia3 In2O3 phase (JCPDS card no. 06-0416). Peaks are quite broad, which demonstrates the nanometric-grained nature of the samples. The absence of a wide peak at about 22º (2θ) related to amorphous silica proves the purity of In2O3 TEM images were taken to assess the quality of both templates (Figure 1a and 1b) and the mesoporous oxide replica. Pure In2O3 samples are highly crystalline, with the typical cubic (byxbyite) structure as observed in XRD patterns. Monocrystalline nano-scaled wires of 5-8 nm in diameter and around 200 nm in length can be observed (Figure 1c)
Figure 1 Mesoporous silica used as a template: KIT-6 a) and SBA-15 b). Detailed of an indium oxide replica of SBA-15 structure. 1. 2. 3. 4. 5. 6.
M.-S. Lee, W. C. Choi, E. K. Kim, C. K. Kim and S.-K. Min, Thin Solid Films, 279 (1996) 1 Prim, E. Pellicer, E. Rossinyol, F. Peiró, A. Cornet and J. R. Morante. Advanced Functional Materials, 17 (2007) 2957. Liang, G. Meng, Y. Lei, F. Phillipp and L. Zhang, Advanced Materials, 13 (2001) 1330. Murali, A. Barve, V. J. Leppert, S. H. Risbud, I. M. Kennedy and H. W. H. Lee, Nano Lett, 1 (2001) 287. Tian, X. Liu, L. Solovyov, Z. Liu, H. Yang, Z. Zhang, S. Xie, F. Zhang, B. Tu, C. Yu, O. Terasaki, D. Zhao. J. Am. Chem. Soc. 126 (2004) 126. Zhao, J. Feng, Q. Huo, N. Melosh, G. H. Fredrickson, B. F. Chmelka, G. D. Stucky, Science 279 (1998) 548
313
Measuring electrical properties of carbon nanotubes using liquid metal immersion, an in situ scanning electron microscopy study H. Strand1, K. Svensson2 and E. Olsson3 1. Department of Physics, Göteborg University, SE-412 96 Göteborg, Sweden 2. Department of Physics and Electrical Engineering, Karlstad University, SE-651 88 Karlstad, Sweden 3. Department of Applied Physics, Chalmers University of Technology, SE-412 96 Göteborg, Sweden [email protected] Keywords: Liquid metal, carbon nanotube, SEM
The electrical properties of nano-materials are of great interest for both science and industry. In particular carbon nanotubes [1] are one of the most studied materials. It is known that the electrical properties of single-walled carbon nanotubes are determined by their chirality [2] and can be either metallic or semiconducting. Experiments have shown the electron transport to be ballistic at room temperature [3]. In multi-walled carbon nanotubes (MWCNTs) the electron transport is more complicated due to the various layers of different chirality, and the dominating transport regime at room temperature is still under some debate. Early low temperature magnetoresistance measurements found evidence of weak localization [4], a correlation effect arising in diffusive systems. These works predicted the transport to be diffusive also at room temperature, as was later confirmed by scanning probe microscopy [3]. All these measurements were performed on substrate deposited MWCNTs. Another very different and exciting experimental approach for room temperature measurements has been introduced by S. Frank et. al. [5]. They mounted MWCNTs on a piezo-controlled tip and used a liquid metal as counter electrode. Immersing a tube by moving the tip then enabled control of the conducting tube length. Applying a voltage (≈100mV) and measuring the current when moving the tip then gave the resistance R as a function of tube length. In the final report [6] it was concluded that the as-produced arc discharge MWCNTs used did display ballistic conduction and electronic mean free paths of the order 10μm. Spurred by these astonishing results we have performed a study of the liquid metal immersion of individual MWCNTs both in air and in situ in a Zeiss Ultra 55 FESEM using an in house developed scanning tunneling microscope (STM) probe. The probe is based on the same principle as the transmission electron microscope (TEM) holder described in [8], now commercially available from [7]. Our MWCNTs was grown by pyrolysis of ferrocene [9] and were known to be diffusive conductors from previous works [10]. We used the model presented in [6] to interpret the conductance traces from our immersion experiments in air. A typical long trace is shown in “Figure 1a-b”. The
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 313–314, DOI: 10.1007/978-3-540-85226-1_157, © Springer-Verlag Berlin Heidelberg 2008
314
obtained resistance per length, ρL, was surprisingly low with, ρL≤120Ω/μm, which is of the same order as previous ballistic claims (ρL≤48Ω/μm [6]). For proper interpretation of our data we repeated the immersion experiments in situ in the SEM. The topological sensitivity of secondary electron imaging enabled us to directly image the liquid metal surface response as the MWCTN was pushed in to it. A SEM-micrograph of the surface is shown in “Figure 1c”, where the bright lower surface is the liquid metal (Hg), showing the formation of an inwards meniscus with a large radius of curvature compared to the length of the MWCNT protruding from the upper, movable, tip. The non-wetting meniscus formation makes the model-calculations invalid, since the model assumes that the tube immersion depth is directly given by the piezo-motion of the tip. We have also found evidence of the formation of a thin layer on the liquid metal surface, a known problem for mercury called “skinning” [11]. The immersion model of [6] seems to have gained acceptance and are used in more recent works such as [12]. Thus we want to stress the importance of monitoring the liquid metal surface response to enable correct modeling of the liquid metal immersion experiment. For this purpose the simultaneous immersion and in situ imaging using SEM has proven to be the ideal tool.
c) 1μm
Figure 1. Electrical measurements of a) the conductance G (G0=2e2/h≈1/12.9kΩ) and b) resistance R as function of piezo movement x, linear fit in b) gives ρL, c) meniscus formation at the liquid metal surface. 1 2 3 4
Iijima, Nature 354 (1991), p. 56-58. M. S. Dresselhaus, G. Dresselhaus and R. Saito, Carbon 33 no. 7 (1995), p. 883-891. A. Bachtold et. al., Phys. Rev. Lett. 84 no. 26 (2000), p. 6082-6085. L. Langer et. al., Phys. Rev. Lett. 76 no. 3 (1996), p. 479-482; A. Bachtold et. al., Nature 379 (1999), p. 673–675; C. Schönenberger et. al., Appl. Phys. A 69 (1999), p. 283-295. 5 S. Frank et. al., Science 280 (1998), p. 1744-1746. 6 P. Poncharal et. al., J. Phys. Chem. B 106 (2002), p. 12104-12118. 7 Nanofactory Instruments AB, www nanofactory.com. 8 K. Svensson et. al., Rev. of Sci. Instr. 74 no. 11 (2003), p. 4945-4947. 9 Produced by H. Pettersson, M. Terrones and N. Grobert, Sussex Nanoscience and Nanotechnology Centre, University of Sussex, England. 10 K. Svensson, H. Olin and E. Olsson, Phys. Rev. Lett. 93 no. 14 (2004). 11 M. C. Wilkinson, Chem. Rev. 72 no. 6 (1972), p. 575-625. 12 H. Kajiura et. al., Chem. Pys. Lett. 398 (2004), p. 476–479; Carbon 43 (2005), p.1317–1339; Appl. Phys. Lett. 86 (2005) art. 122106
315
TEM characterization of biogenic metal nanoparticles E.I. Suvorova1,3, P.A. Buffat1, H. Veeramani1, J. Sharp1, E. Schofield2, J. Bargar2, and R. Bernier-Latmani1 1. Environmental Microbiology Laboratory, Ecole Polytechnique Fédérale de Lausanne, Station 6, CH-1015 Lausanne, Switzerland 2. Stanford Synchrotron Radiation Laboratory, Menlo Park, CA 3. Institute of Crystallography RAS, Leninsky pr., 59, Moscow 119333, Russia elena.suvorova @epfl.ch Keywords: Cr and U oxides nanoparticles, microbial reduction, HRTEM and X-ray EDS analysis
Biogenic nanoparticles formed by microbial reduction of uranyl and chromate were investigated in order to understand the mechanism and to design strategies for the bioremediation of Cr (VI) and U (VI) contaminated groundwater. Analysis of composition, structure, morphology and sizes of particles were carried out in a FEI CM300UT FEG electron microscope in TEM/HRTEM/Electron diffraction/STEM/EDS mode. The images were recorded on a Gatan 797 slow scan CCD camera and processed with the Gatan Digital Micrograph 3.11.1 software, INCA (Oxford) and JEMS package [1]. Low intensity illumination conditions were used to record the HRTEM images. Element-specific short-range structural and chemical information about the U coordination environment was derived from the Extended Xray Adsorption Fine Structure (EXAFS) spectra collected at room temperature or at 77K at the Stanford Synchrotron Radiation Laboratory and processed with the software package SIXPACK. The microbial reduction of uranyl and chromate, the toxic and highly soluble forms of the metals, to sparingly soluble Cr (III) as Cr (III) hydroxide/oxide/phosphate and U(IV) as UO2 was observed. Uraninite, UO2, a face-centered cubic mineral, occurred as nanoparticles, (Figure 1). Their size did not exceed 4.0±0.2 nm in diameter. The addition of Mn or Mg cations during the reduction process resulted in a reduction in uraninite particle size: their diameter did not exceed 3.0 ± 0.2 nm. Cr(VI) reduction was studied in the presence and absence of Fe(III) and yielded a non-crystalline precipitate. STEM and EDS methods were used to characterize this material. Previous work has shown that a mixed FexCry(OH)3 phase was formed when both Cr(VI) and Fe(III) were present [2]. The present STEM/EDS data support two observations: (i) a Cr(III)-only phase was associated with the bacterial surface (Figure 2a) and (ii) elemental maps of particle aggregates away from the bacterial surface suggested that several Cr and Fe phases, for instance CrPO4, Cr2O3, Cr(OH)3, FePO4 and Fe2O3 could form and coexist (Figure 2b). 1. 2.
P. Stadelmann, JEMS. http://cime.epfl.ch, 2008. C.M. Hansel, B.W. Wielinga, S. Fendorf. Geochimica et Cosmochimica Acta, Vol. 67 (2003), pp. 401–412.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 315–316, DOI: 10.1007/978-3-540-85226-1_158, © Springer-Verlag Berlin Heidelberg 2008
316
Figure 1. TEM (a), SAED (b), HRTEM (c), and a diffractogram (d) taken from the UO2 nanoparticles. Figure 2. STEM images and element maps of Cr (III) precipitates on the bacterial surface (a) and an agglomerate with mixture of Fe (III) and Cr (III) particles (b).
317
On the structure of VxOy supported on multiwalled carbon nanotubes D. Wang1, J.-P. Tessonnier1, M. Willinger1,2, C. Hess, D.S. Su1, R. Schlögl1 1. Abteilung Anorganishe Chemie, Fritz-Haber-Institut der Max-Planck-Gesellschaft, Faradayweg 4-6, D-14195 Berlin, Germany 2. Department of Chemistry, CICECO, University of Aveiro 3810-193 Aveiro, Portugal [email protected] Keywords: Vanadium oxide, catalysis, carbon nanotubes, TEM
Supported highly dispersed Vanadium oxides are of great interests for the high activity in selective oxidation of small alkanes (propane, butane) [1]. CNTs are widely used in heterogeneous catalysis as support as it is possible to manipulate them by specific chemical and thermal treatments aimed to tune the surface chemistry [2]. By incipient wetness impregnation with vanadium oxide triisopropoxide in isopropanol, highly dispersed vanadium oxide on commercial carbon nanotubes (Baytubes) with loadings of 3, 10 and 20 wt. % V were synthesized. Catalytic reactions were performed on small amounts of catalyst directly mounted onto a gold TEM grid in a microreactor, allowing direct correlation between structure and catalytic behaviors. The catalysts with lower vanadium loading show a high initial activity at 400°C but deactivate quickly. The VxOy/MWCNTs samples with different loadings were investigated by (HR)TEM, EDX ,EELS, XPS and Raman spectroscopy. The HRTEM image from 3 wt.% VxOy/CNTs (Figure 1a) looks very similar to the pure CNTs, while the EDX spectrum from an area of about 1 μm2 shows confirm the V quantity (2.8 wt. %) in agreement with the nominal value. The observation indicates two-dimensionally dispersed VxOy species both inside and outside of the CNTs. With increase of V loading to 10 wt. %, the morphology of CNTs doesn’t change noticeably and the EDX spectrum from large area confirms the V loading (12.9 wt.%). However, aggregated islands are more frequently observed, as shown in Figure 1b with corresponding local EDX spectrum in the inset. These islands are mostly flattened and extend along CNTs surfaces with the thickness of 1-2 nm. Such aggregation becomes more prominent for 20 wt. % VxOy/CNTs. V oxides form continuous aggregates over large area on the surface of CNTs or fill the inner space within the CNTs. After test in oxidation of propane to propylene at 400°C, the CNTs support was destroyed for all the catalysts and the TEM image shows that a considerable amount of V oxides form crystals. Representatively, Figures 2a, 2b and 2c show the overview image, selected area diffraction pattern and the HRTEM image of the 10 wt. % VxOy/CNTs after the reaction, respectively. The HRTEM image shows the lattice spacing other than V2O5 while the diffraction pattern is in good agreement with the simulated V2O5 diffractions (inset in Figure 5b). Such result implies that the main structure of the V oxides after the reaction is V2O5 and some suboxides phases may coexist on the surface. S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 317–318, DOI: 10.1007/978-3-540-85226-1_159, © Springer-Verlag Berlin Heidelberg 2008
318
The oxidation states of V oxides for as prepared catalysts and those after the reaction were also studied by EELS. From the ELNES of V L2,3 edge and O Kedge, an oxidation state lower than 5+ can be deduced for the 3 % V catalyst. The as prepared catalysts with higher loading have varying V oxidation states in different areas. After test in oxidation of propane, the aggregated V oxides show exclusively an oxidation state close to 5+, in agreement with the electron diffraction result. In summary, highly dispersed VxOy species are highly active in selective oxidation of small alkanes. Deactivation is attributed to the formation of bulky vanadium oxides. How to stabilize the VxOy species is essential for optimization of the catalysts. 1 2 3
C. Hess, U. Wild and R. Schloegl, Microporous Mesoporous Mater. 95 (2006), p. 339. W. Xia, Y. Wang, R. Bergstraesser, S. Kundu and M. Muhler, Appl. Sur. Sci. 254 (2007), p. 247. The authors acknowledge financial support by SFB 546 “Transition Metal Oxide Aggregates.”
Figure 1 HRTEM images of VxOy/MWCNTs a) with a loading of 3 wt% V and b) 10 wt% V (right). The formation of VxOy islands is confirmed by EDX.
Figure 2 a) Overview image, b) selected area diffraction pattern together with the simulated pattern and c) HRTEM image of the 10 wt% V/MWCNT catalyst after reaction, respectively.
319
Hexahedral nano-cementites catalysing the growth of carbon nanohelices J.H. Xia1,3, X. Jiang1,3, C.L. Jia2 and C. Dong3 1. Institute of Materials Engineering, University of Siegen, Paul-Bonatz-Str. 9-11, 57076 Siegen, Germany 2. Institute of Solid State Research and Ernst Ruska Centre for Microscopy and Spectroscopy with Electrons, Research Centre Jülich, D-52425 Jülich, Germany State 3. Key Laboratory of Materials Modification & Department of Materials Engineering, Dalian University of Technology, Dalian 116024, P. R. China j [email protected] Keywords: Carbon nanohelices, hexahedral nano-cementites, growth mechanism
Helical carbon structures (fibers, tubes, etc) have attracted considerable attention of research owing to their attractive morphology and properties [1,2]. Carbon nanohelix (CNH) is one type in the helical family, which has been grown on iron needles using microwave plasma assisted chemical vapor deposition (MPCVD) [3]. To explore the formation mechanism of CNH, systematic investigations on the catalyst particle are carried out by means of scanning electron microscopy (SEM) and transmission electron microscopy (TEM). The catalyst is identified to be single crystalline cementite (Fe3C) particle at the tip of each CNH. The Fe3C particles show a general morphology of hexahedron with six (different) crystallographic planes as the surface planes, which is determined by shape fitting with the series of TEM images (Figure 1.). The different catalytic effect of different crystallographic surface planes produces an anisotropic growth on the front surface of the carbon nanostructure, which results in a rotation of the cementite particles. The rotating particles catalyse the growth of the carbon nanostructure in a helix way. The schematic growth model is shown in Figure 2.
1. 2. 3.
S. Amelinckx, X. B. Zhang, D. Bernaerts, X. F. Zhang, V. Ivanov and J. B. Nagy, Science 265, 635 (1994). S. M. Yang, X. Q. Chen and S. Motojima, Appl. Phys. Lett. 81, 3567 (2002). G. Y. Zhang, X. Jiang, and E. G. Wang, Appl. Phys. Lett. 84, 2646 (2004).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 319–320, DOI: 10.1007/978-3-540-85226-1_160, © Springer-Verlag Berlin Heidelberg 2008
320
Figure 1. (Up left) Series of TEM images and corresponding diffraction patterns of Fe3C catalyst particles recorded along different crystallographic directions. In (a)-(d) the images and diffraction patterns are obtained by tilting a particle around the [110] axis (arrows in diffraction patterns). In (e) and (f) the images and diffraction patterns are recorded by tilting around the [001] axis. Details are described in main text. A hexahedron model of the particle is shown in (g) and its projections are shown accompanying the image series. Figure 2. (Up right) The schematic growth model of the nanohelices.
321
Investigation of organic/inorganic interfaces using nano-analytical transmission electron microscopy V. Jantou1, M.A. Horton2 and D.W. McComb1 1. Dept. of Materials, Imperial College London and London Centre for Nanotechnology 2. Dept. of Medicine, University College London and London Centre for Nanotechnology. d [email protected] Keywords: EELS, FIB milling, apatite, collagen
The impact of long-term health problems due to skeletal disorders, such as osteoporosis and arthritis, is increasing with the ageing of modern populations. Bone pathologies have a critical effect on the mechanical properties of bone, which are intimately linked to its highly complex hierarchical structure. However, despite decades of investigation, bone nanostructure (essentially made of collagen fibrils and apatite crystals) is not well understood. The exact structure and chemistry of bone crystals and their location with respect to collagen is still debated. The currently accepted 2D model [1] states that the collagen molecules are arranged in a quarter-stagger fashion, creating gap and overlap regions; the crystals are thought to be located inside the gap zone, giving rise to a periodic contrast in electron micrographs of bone collagen. In order to gain a better understanding of the relationship between the apatite and collagen, it is crucial to study the composition and bonding along collagen fibrils. In the present work, the organic/inorganic interface in mineralised ivory dentin, which acts as a good model for bone, was studied using analytical scanning transmission electron microscopy (STEM), with samples prepared using focused ion beam (FIB) milling as an alternative technique to ultramicrotomy. A monochromated FEG(S)TEM (FEI Titan 80-300) instrument was used, providing both high-resolution imaging and spectroscopy capabilities using electron energy-loss spectroscopy (EELS) and energy-filtering TEM (EFTEM). The Titan offers a spatial resolution <0.14 nm and an energy resolution <0.2 eV. A clear advantage of FIB milling over ultramicrotomy is that dehydration, embedding and section flotation can be obviated, thus reducing both physical and chemical damage to the specimen prior to examination. FIB milling has other significant advantages over ultramicrotomy, such as site-specificity and the ability to image whilst milling, which provides greater control over the final section thickness. The characteristic periodic contrast of collagen fibrils was visible in FIB sections without the need for any chemical staining, contrary to ultramicrotomed sections. Consequently, the origin of the collagen periodic contrast can now be properly investigated by performing compositional analysis on the nanometer scale, without the chemical complications arising from the sample preparation procedure. EELS and EFTEM mapping of P, O and Ca, the principal constituents of apatite crystals, and C, the major component of the organic phase, are currently being carried
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 321–322, DOI: 10.1007/978-3-540-85226-1_161, © Springer-Verlag Berlin Heidelberg 2008
322
out, and data is acquired along and across collagen fibrils. By studying not only the position and shape of a peak, but also the fine structure after each edge onset, termed electron energy-loss near-edge structure (ELNES), the atomic environment of a particular species can be determined [3], allowing differently bonded Ca or C atoms to be distinguished. It is the first time that some of the fundamental questions of mineralised tissues can be approached using nano-analytical TEM, which will ultimately provide crucial information regarding the mechanisms of bio-mineralization and how it is altered in diseases. 1. 2. 3.
Weiner S. and Traub W., FASEB Journal 6 (1992), p. 879. Egerton, R.F., NY-London Plenum Press (1996). The authors gratefully acknowledge the Department of Materials, Imperial College London, and University College London (Dr. Mortimer and Mrs. Theresa Sackler Trust).
Figure 1. BF-TEM images of FIB milled and ultramicrotomed sections along (long.) and across (trans.) collagen fibrils. The dotted encircled region defines the crosssectional profile of a collagen fibril.
Figure 2. STEM-EELS line profile across a collagen fibril on a FIB milled section. The spectra were recorded at 100kV, with an energy resolution of 0.6eV, a dispersion of 0.2eV/pixel, and convergence/collection semi-angles of 10.5mrads and 11.8 mrads respectively.
323
Cationic ordering and interface effects in superlattices and nanostructured materials P. Boullay, W.C. Sheets, W. Prellier, E.-L. Rautama, A.K. Kundu, V. Caignaert, B. Mercey and B. Raveau Laboratoire CRISMAT, UMR 6508 CNRS/ENSICAEN, 6 Bd Maréchal Juin, 14050 Caen Cedex 4, France philippe.boullay@ensicaen fr Keywords: perovskites, HRTEM, heterostructures, domain texture
Thin film methods offer a versatile approach to overcome the natural preference for disorder or low-dimensional ordering in certain materials by controlling the location of cations in tailored oxide multilayers. Artificial heterostructures have hence been utilized to probe how interlayer coupling and cation ordering at the interface affect magnetic or transport properties. Recently, it was shown that LaTiO/SrTiO3 superlattices exhibit metallic conductivity, similar to a bulk solid solution of La1−xSrxTiO3, even though the heterostructure is based on two insulators [1]. In this contribution, a series of highquality (LaVO3)6m(SrVO3)m superlattices (Figure 1) with a nominal composition close to La6/7Sr1/7VO3 has been grown on [001]-oriented SrTiO3 substrates using standard pulsed-laser deposition [2]. When m=1, the bulk-like insulating resistivity of La6/7Sr1/7VO3 is obtained while for m≥2 the superlattices display a metallic behaviour. The comparison of the superlattice periodicity with the known coherence length of charge carriers across the interface of perovskite oxide heterostructures is used to understand this insulator-metal transition. The magnetic and transport properties of manganites and cobaltites with the perovskite structure have been the object of numerous studies. A modification of the cation ordering in such strongly correlated electronic oxides can also affect properties. From this perspective, our recent study of the perovskite La0 5Ba0 5CoO3 has allowed three forms to be isolated. Besides the known disordered La0 5Ba0 5CoO3 and layered 112-type LaBaCo2O6 forms, a third nanoscale-ordered form is obtained [3]. This new form presents a specific nanostructure that consists of 112-type 90° oriented domains fitted into each other at a nanometer scale in order to form a 3D domain texture [4] that induces large strains in the material (Figure 2). Differently from the other forms, this latter is a hard ferromagnet due to the strains which may pin domain walls, preventing the reversal of the spins in a magnetic field illustrating that the atomic-scale lattice distortions are coupled to the magnetic and electronic degrees of freedom. 1. 2. 3. 4.
A. Ohtomo, D.A. Muller, J.L. Grazul and H.Y. Hwang, Nature 419 (2002), 378. W.C. Sheets, B. Mercey and W. Prellier, Appl. Phys. Lett. 91 (2007), 192102. E-L. Rautama, P. Boullay, A.K. Kundu, V. Caignaert, V. Pralong, M. Karppinen and B. Raveau, Chem. Mat. (2008), in press. M.A. Alario-Franco, M.J.R. Henche, M. Vallet, J.M. Gonzalez-Calbet, J.C. Grenier, A. Wattiaux, P. Hagenmuller, J. Solid State Chem. 46 (1983), 23.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 323–324, DOI: 10.1007/978-3-540-85226-1_162, © Springer-Verlag Berlin Heidelberg 2008
324
Figure 1. Cross-sectional HRTEM image obtained for a metallic (LaVO3)17(SrVO3)3 superlattice with a periodicity of ~78Å.
Figure 2. Bright-Field images obtained for the nanostructured LaBaCo2O6. A mottled contrast consisting of curved and interpenetrated dark segments is observed and related to the existence of strain fields induced by the 3D texture at a nanometer scale.
325
Strain in SrTiO3 layers embedded in a scandate/titanate multilayer system D. Ávila1, M. Boese1, T. Heeg2, J. Schubert2 and M. Luysberg1 1. Institut für Festkörperforschung und Ernst Ruska-Centrum, Forschunszentrum Jülich, 52425 Jülich, Germany 2. Institut für Bio- und Nanosysteme, Forschunszentrum Jülich, 52425 Jülich, Germany [email protected] Keywords: SrTiO3, strain
Deposition of earth alkali titanate thin films on different substrates allows to tune the strain and, as consequence, their dielectric properties. In this sense, the large range of available lattice constants in rare earth scandates make them very useful candidates to serve as substrate materials for epitaxial growth. In this work we have employed aberration corrected high-resolution transmission electron microscopy (HRTEM) to quantify the strain in different scandate/titanate multilayers by using the geometrical phase analysis method [1]. Besides, we applied electron energy loss spectroscopy (EELS) and ab initio calculations to obtain information about the effect of the strain on the electronic structure of these materials. The multilayers of DyScO3/SrTiO3 (DSO/STO) and GdScO3/SrTiO3 were grown by Pulsed Laser Deposition (PLD) using GdcSO3 or DyScO3 substrates [2,3]. The HRTEM study was carried out in an image corrected CM200 microscope. EEL spectra were recorded in a probe corrected Titan microscope. Ab-initio calculations were performed with the Feff8.2 code based on the real space multiple scattering method. Exit-plane wave reconstruction [4] was utilized for the analysis of DyScO3/SrTiO3 multilayers recording a focus series of 20 images with a focal increment of 1.7 nm. The phase image shown in Fig. 1 is analysed with the geometric phase analysis. Linescans corresponding to the red frame in Fig 1 have been performed for the in plane (ip, parallel to the interface), and out of plane (op, growth direction) lattice constants, respectively. Clearly a tetragonal distortion of the STO layers is revealed, which amounts to a maximum 2% of tensile strain, translating to 8 pm smaller lattice parameter of SrTiO3 compared with the in plane lattice parameter of 395 pm= aDSO. EEL spectra have been recorded for the strained STO layers within the multilayer system (red curve in Fig. 2). Compared to a reference spectrum obtained from a STO substrate, a significant smaller splitting of the L3 edge is detected. In cubic SrTiO3 the Ti is surrounded by six O forming a regular octahedron with Ti-O distances 0.195 nm. However, under tensile strain this octahedron is distorted yielding an average distance Ti-O 0.196 nm. This enlargement of the distances produces a weaker crystal field, which results in a smaller splitting. The reduced crystal field splitting is reproduced by ab initio calculations of the Ti L3 edges using the Feff8.2 code (see Fig. 2). Calculations of the L3 edge for different strain situations reveal, that the splitting of the L3 linearly decreases with increasing strain.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 325–326, DOI: 10.1007/978-3-540-85226-1_163, © Springer-Verlag Berlin Heidelberg 2008
326
1. 2.
M. J. Hytch, E. Snoeck, R. Kilaas, R. Ultramicroscopy 74 (1998) T. Heeg, M. Wagner, J. Schubert, Ch. Buchal, M. Boese, M. Luysberg, E. Cicerrella, J.L. Freeouf, Microelectronic Engineering 80, (2005) 150 3. M. Boese, T. Heeg, J. Schubert, M. Luysberg, J. Mat. Sci. 41, (2006) 4434 4. A. Thust, W. Coene, M. Op de Beeck, and D. Van Dyck, Ultramicroscopy 64 (1996), 211230 *present address: Carl Zeiss NTS GmbH, Carl-Zeiss Str. 56, 73447 Oberkochen STO
DSO
STO
DSO
STO ip
DSO op
STO STO
DSO
2 nm
Figure 1: Phase image obtained from a through focus series of STO/DSO multilayers. The linescans shown on the right hand side correspond to the in plane and out of plane lattice parameters obtained from corresponding geometrical phase images. The in plane lattice parameter shows only small variations, whereas the out of plane parameter varies by 2% across the layer system. Cubic 40
30
Ti-O: 1.95
ΔE = 2.22 eV ΔE = 2.01 eV
20
10
experimental
Strained
ΔE = 2.12 eV ΔE = 2.01 eV
0 455
Feff calculations 456
457
458
459
Ti-Oav.: 1.96
460
Energy Loss (eV )
Figure 2: Experimental and calculated EEL spectra of the Ti L3 edge obtained for cubic SrTiO3 (black curves) and tensilely strained SrTiO3 (red curves). In the strained case, i.e. the in plane lattice parameter resumes the value of DSO, the average Ti-O bond is by 0.01 Å larger, resulting in a smaller crystal field splitting.
327
Anisotropic growth of CGO islands on the (001)-LaAlO3 surface A. Benedetti, M. Gibert, F. Sandiumenge, T. Puig and X. Obradors Institut de Ciència de Materials de Barcelona, CSIC, Campus de la UAB, 08193 Bellaterra, Catalonia, Spain [email protected] Keywords: nanohuts, CGO, chemical solution deposition
Chemical solution deposition (CSD) has emerged as a very competitive, low cost and easily scaleable technique for obtaining highly epitaxial multilayered structures, and very recently its high potential for the generation of high quality self assembled templates has been also demonstrated [1]. As a further step, in this contribution we focus on the correlation between shape anisotropy and anisotropic mismatch of Ce1-xGdxOy, x=0.1, (CGO) islands grown on (001)-LaAlO3 (LAO) by CSD, investigated using x-ray diffraction pole-figure analysis, atomic force microscopy (AFM), and high resolution electron microscopy (HREM). Anisotropic mismatch on an isotropic substrate surface in the CGO-LAO system is promoted by the strong sensitivity of island orientation to growth conditions. In particular, we have recently demonstrated that the usual (001)[110]CGO//(001)[100]LAO epitaxial relationship can be replaced by the (110)[1-10]CGO//(001)[100]LAO one [1]. Fig. 1(a) is an AFM image of highly anisotropic nano-huts grown at reduced pO2, exhibiting the (110)[1-10]CGO//(001)[100]LAO epitaxial relationship. This configuration involves an extremely high misfit direction (<100>CGO//<100>LAO, ε~-30%) coexisting with a low misfit direction ([1-10]CGO//[100]LAO, ε ~-1%). Fig. 1(b) shows a HREM cross sectional view of a nano-hut, viewed along the [1-10]CGO direction, i.e., the long direction of nano-huts in Fig. 1(a). The nano-huts are narrower along the higher mismatch strain direction. Despite the huge mismatch, overall the image demonstrates good crystallinity (image simulations indicate that white dots correspond to atom columns of the fluorite-type CGO structure), though the inner region exhibits a change in contrast due to strain localization, very likely associated with the solid-phase growth mechanism of the islands. The interface appears structurally incoherent, which can be understood taking into account the huge mismatch strain. Since the most likely interfacial component of the Burgers vector for CGO is ½<100> [2], full relaxation of such a huge mismatch strain requires a dislocation spacing of 0.9 nm, i.e., a dislocation every other unit cell. This distance agrees well with what we experimentally measured by Fourier analysis (1 - 1.1 nm), indicating that nearly full relaxation takes place. Insights into the strain state within the island where obtained from strain maps obtained by the geometric phase method [3], using an undistorted area of the island as a reference. Images 1(c) and 1(d) display the strain tensor components εxx and εyy, where x and y are parallel and normal to the interface, respectively. With the exception of the central defective region, both strain components, in particular εxx which is more
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 327–328, DOI: 10.1007/978-3-540-85226-1_164, © Springer-Verlag Berlin Heidelberg 2008
328
sensitive to in-plane strains, reveal a rather homogeneous strain distribution, with values comprised in the range -0.01< ε<0.01 which can hardly be associated with an elastically strained island as a consequence of such a large mismatch. Interestingly, despite the high degree of relaxation the bottom corners of the island (encircled in Fig. 1(b)) show some degree of disorder and are lifted from the substrate surface, suggesting that besides full relaxation within the islands, structural difference with the substrate may represent an additional obstacle to island growth. 1. 2. 3.
M. Gibert, T. Puig, X. Obradors, A. Benedetti, F. Sandiumenge, R. Hühne, Adv. Mater. 19 (2007) pp. 3937–3942 A. Cavallaro, F. Sandiumenge, J. Gazquez, T. Puig, X. Obradors, J. Arbiol, H. C. Freyhardt, Adv. Function. Nanomat. 16 (2006) pp.1363–1372 M. J. Hÿtch, E. Snoeck, R. Kilaas, Ultramicroscopy 74, (1998) pp. 131–146
a)
c))
b)
d)
Figure 1. (a) AFM image of CGO nano-huts oriented along two mutually perpendicular directions of the (001)-LAO surface; (b) HREM cross sectional image of a nano-hut viewed along the [1-10]CGO or [100]LAO directions. The interface shown in the image corresponds to a mismatch strain of ~30%. (c) εxx (d) εyy components of the strain versor within the island. The white numbers indicate the corresponding levels of strain.
329
Diffraction contrast imaging and high resolution transmission electron microscopy of multiferroic thin films and heterostructures B.I. Birajdar, I. Vrejoiu, X.S. Gao, B.J. Rodriguez, M. Alexe, and D. Hesse Max Planck Institute of Microstructure Physics, Weinberg 2, D-06120 Halle (Saale), Germany [email protected] Keywords: transmission electron microscopy, multiferroics, epitaxial strain
Multiferroic materials exhibit simultaneous ferroelectric and ferromagnetic properties and are extensively studied because of their potential applications in multifunctional devices as well as for the understanding of the physics underlying multiferroicity [1]. The properties of these materials are influenced by their crystal structure and microstructural properties like strain, dislocations and domain boundaries, which can all be uniquely studied using transmission electron microscopy (TEM). Intrinsically multiferroic films and extrinsically multiferroic heterostructures and their components in the form of (1) BiFeO3 (BFO) epitaxial thin films (sample 1), (2) CoFe2O4 (CFO) epitaxial thin films (sample 2), (3) multilayers of (La,Sr)MnO3 (LSMO) and Pb(Zr,Ti)O3 (PZT) (sample 3), and (4) nanostructures of CFO (sample 4) (see Figure 1) were synthesised by pulsed laser deposition (PLD). Their microstructure was investigated using diffraction contrast imaging with a CM20T TEM operated at 200 kV, high resolution TEM [2] using a Jeol 4010 operated at 400 kV, and piezoresponse (PFM) and magnetic (MFM) force microscopies. Macroscopic ferroelectric and magnetic properties were measured by standard methods. The TEM bright field image of sample 1 in cross-section (Figure 1a) shows a 180 nm thick BFO film and a 50 nm thick SrRuO3 (SRO) bottom electrode on DyScO3 (DSO) (110) substrate. The films are single phase, show crystalline contrast and have sharp interfaces. The microstructure of the BFO films was extremely sensitive to the growth conditions (annealing temperature and oxygen pressure) and slight deviations from the optimum conditions led to secondary phases, in agreement with previous reports. The BFO film of sample 1 revealed a multidomain structure (Figure 1e) (cf. [3]), and similar domain structures were observed using PFM (Figure 1f). Diffraction patterns consisted of split spots confirming the formation of domains. Sample 1 has a remnant polarisation of about 55 μC/cm2 at room temperature and 1 kHz, similar to the value given in the recent literature reports [3], which is attributed to the high structural quality of these films. The TEM bright field image of sample 2 in cross section (Figure 1b) shows a 120 nm thick CFO film and a 20 nm thick SRO electrode on a STO substrate. The CFO film is epitaxial and single phase but has a high density of structural defects. In some films dislocations were observed at the SRO-CFO interface. (Investigations of the magnetic domain structure of the CFO films using plan-view TEM and MFM are under way).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 329–330, DOI: 10.1007/978-3-540-85226-1_165, © Springer-Verlag Berlin Heidelberg 2008
330
Indexing of [010] diffraction patterns showed a similar in-plane lattice parameter of the CFO film, the SRO film, and the STO substrate indicating strained epitaxial growth. The out-of-plane lattice parameter of CFO is larger than its bulk value leading to c/a ratio of 1.08.The CFO films appears to be in compressive stress. Sample 2 showed inplane and out-of-plane values of the remnant magnetization of 266 and 33 emu/cm3 respectively, which is comparable with recent reports in the literature [4]. Sample 3 is a graded heterostructure consisting of ferromagnetic LSMO films sandwiched between ferroelectric PZT films of increasing Zr content (Figure 1c) which exert in-plane tensile stress on the LSMO layers significantly altering their magnetic properties [5]. Sample 4 is an array of 35 nm large CFO islands (Figure 1d), synthesised using a deposition mask made from anodic aluminum oxide (AAO) [6]. Because of their reduced dimension, these CFO islands are expected to be under strain yielding significant changes in the ferromagnetic properties. The measurement of these properties is however challenging because of the complex design of nanostructured arrays. Quantitative analysis of the strain in the multilayers (sample 3) and nanostructures (sample 4) using HREM and geometric phase imaging (cf. [7]), as well as the application of other analytical techniques like EDX and EELS are under way. 1. 2. 3. 4. 5. 6. 7.
S.-W. Cheong and M. Mostovoy, Nature Materials 6 (2007) 13. Help by Dr. S. Senz and Dr. N. D. Zakharov in HREM is gratefully acknowledged. Y.-H. Chu et al., Adv. Mater. 18 (2006) 2307 W. Huang et al., Appl. Phys. Lett. 89 (2006) 262506 I. Vrejoiu et al., submitted to Appl. Phys. Lett. X. S. Gao et al., submitted to Int. Symp. on Integrated Ferroelectrics (ISIF), Singapore 2008. M.-W. Chu et al., Nature Materials 3 (2004) 87.
Figure 1. (a-d) TEM bright-field (cross section) images of samples 1-4, (e-f) TEM bright-field (plan-view) and in-plane PFM amplitude images of sample 1 showing a multidomain structure.
331
Imaging of compositional defects at silicide-silicon interfaces using aberration corrected HAADF M. Falke1, U. Falke2, P. Wang2, A. Bleloch2 1. Institute of Physics, Chemnitz University of Technology, 09107 Chemnitz, Germany 2. SuperSTEM Laboratory, Daresbury, Cheshire, WA4 4AD, U.K. [email protected] Keywords: interfaces, HAADF, aberration correction,
Silicide-silicon interfaces were studied at the superSTEM Laboratory using aberration corrected dedicated STEM at 100kV. With suitable samples the resolution of about 0.1 nm allows compositional defects of atomic dimension to be visualised in high angle annular dark field (HAADF) images. Cubic metal silicides grown epitaxially on cubic (001) Si were chosen for these investigations, since, in case of bulk crystals on a [110] zone axis, only pure metal and pure silicon columns face the electron beam. At the interface however, strain and differences in chemical solubility can produce various, mostly periodically appearing one-dimensional defects. To evaluate the defect structure it is first necessary to understand the more or less undisturbed interface. We reported the interface structures found for cubic NiSi2 and CoSi2 on Si (001) [1,2]. Here we report some defects which disturb this interface structure and are usually found close to steps or local changes in composition. The periodic nature of the defects, shown here means that they could be described as compositional interface reconstructions. Sometimes the defect structure can be derived intuitively from the HAADF contrast, see e.g. Figure 1 showing missing metal columns which appear as dark triangles at the interface and Figure 2 showing that metal and silicon columns seem to exchange their places at a regular distance of a few unit cells. Image simulation and comparison with thickness and imaging data can reveal more about the real content of metal and silicon in the disturbed columns. Figure 3 shows the interface of a mixed NiSi/NiSi2 film on Silicon which was alloyed with 7% of platinum and annealed at 700 °C. Since Pt is not soluble in NiSi2 but easily soluble in NiSi the remaining Pt segregates at periodic sites at the NiSi2/Si interface. This effect is found close to nickel monosilicide crystallites, which contain Pt evenly distributed. Here again judging simply from the HAADF the bright spots arranged regularly at the interface are very likely to arise from Pt rich atomic columns. Image simulations support this and reveal more information about the Pt content. In summary we show how suitable and powerful aberration corrected HAADF imaging in a dedicated STEM is to study metal silicon combinations which are relevant to the semiconductor industry and which provide very interesting model interfaces. 1. 2. 3.
U. Falke, A. Bleloch, M. Falke, and S. Teichert, Phys. Rev. Lett. V92, N11 (2004) 116103. M. Falke, U. Falke, A. Bleloch et al., Appl. Phys. Lett. 86 (2005) 203103. We would like to acknowledge financial support from DAAD Project Number D/07/09995.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 331–332, DOI: 10.1007/978-3-540-85226-1_166, © Springer-Verlag Berlin Heidelberg 2008
332
Figure 1. Metal columns missing every fifth unit cell in HAADF contrast.
Figure 2. Periodically appearing compositional changes were observed close to interface steps in CoSi2 / Si samples. The inset shows an HAADF image simulation (E.J. Kirkland, Advanced Computing in Electron Microscopy, ISBN 0-306-45936-1).
Figure 3. HAADF image of the Si-A- to a NiSi2-B-type interface, containing Pt-rich columns.
333
Characterization of nanometric oxide particles extracted from a steel surface onto a carbon replica P. Haghi-Ashtiani1, A. Ollivier2 and M.-L. Giorgi2 1. Laboratoire de Mécanique des Sols, Structures et Matériaux, CNRS UMR 8579, École Centrale Paris, Grande Voie des Vignes, 92295 Châtenay-Malabry, France 2. Laboratoire de Génie des Procédés et Matériaux, École Centrale Paris, Grande Voie des Vignes, 92295 Châtenay-Malabry, France paul haghi-ashtiani@ecp fr Keywords: replica TEM preparation, electron diffraction, selective oxidation
In steel industry, after cold rolling, steel sheets are annealed in an atmosphere of N2 and H2 (5 to 15 vol.%) in order to recrystallize the steel substrate. During annealing, the less noble alloying elements such as Si and Mn segregate to the surface where they form discrete oxide particles [1]. The main objective of the work presented here is to gain better understanding of the formation of these oxide particles. The annealing experiments were performed on a ternary alloy containing Fe, Si (0.094 wt.%) and Mn (0.492 wt.%), the principal impurities being C (less than 10 ppm), N, O and S (less than 5 ppm). Before the experiments, the substrates were mirrorpolished up to 1 µm with diamond paste. The specimens were annealed in the quartz chamber of an infrared radiation furnace (Ulvac Sinku-Riko) with a temperature profile in line with the industrial practice (Figure 1). The furnace gas atmosphere consists of a commercial high purity N2 and 5 vol.% H2 mixture containing a controlled partial pressure of water (12.8 Pa). After annealing, the laboratory steel surface is covered with small spherical particles (Figure 2a). The particles are extracted from the steel surface using the double replica methodology (Figure 2b): 1) in the first step, the particles are extracted onto a cellulose acetate polymer film, and 2) in the second step, the polymer film covered by the particles is coated with an approximately 20 nm-thick layer of carbon. This double replica is then inserted in a copper grid and the polymer film is dissolved carefully in acetone. The chemical nature of the particles is determined by electron diffraction in the transmission electron microscope (TEM JEOL 1200 EX) at 120 kV, using selected area diffraction and conventional bright field and dark field techniques. The experimental diffraction patterns are compared with theoretical ones in order to determine the chemical nature and orientation of the particle (Figure 3). The crystal structure of the possible oxides (lattice parameters and atom positions) is found in the Inorganic Crystal Structure Database (ICSD) [2] (Figure 3a). Based on the crystal parameters, theoretical electron diffraction patterns are calculated by means of the Java Electron Microscopy Simulation (JEMS) software [3] (Figure 3b). The particles present on the replica contain Mn2SiO4 (Figure 3c) and MnO. Conventional bright and dark field techniques reveal that the spherical particles can be
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 333–334, DOI: 10.1007/978-3-540-85226-1_167, © Springer-Verlag Berlin Heidelberg 2008
334
composed of either several oxides or several grains of the same oxide with different orientations (Figure 4). This result illustrates the complexity of the oxides’ nucleation and growth within a particle. 1. 2. 3. 4.
A.R. Marder, Prog. Mater. Sci. 45 (2000), p.191. Fachinformationszentrum Karlsruhe, National Institute of Standards and Technology: Inorganic Crystal Structure Database ICDS, Karlsruhe, Germany, 2006. P. Stadelmann, Java Electron Microscopy Simulation (JEMS) software, CIME-EPFL, École Polytechnique Fédérale de Lausanne, Switzerland, 1999-2006. The authors are extremely grateful to Natural Resources Canada's CANMET-Materials Technology Laboratory for sharing their extraction replica methodology.
1000
T (°C)
800
Fig. 2a)
600
400
200
0 0
100
200
300
400
500
t (s)
Figure 1. Temperature profile
Fig. 3a)
Fig. 2b)
Figure 2. a) Specimen after annealing, b) TEM image of this specimen’s replica
Fig. 3b)
Fig. 3c)
Figure 3. a) Crystal of Mn2SiO4 in the [100] orientation, b) simulation for Mn2SiO4 in the [100] electron incidence, and c) experimental electron diffraction micrograph obtained
Fig. 4a)
Fig. 4b)
Fig. 4c)
Fig. 4d)
Figure 4. a) Bright and b), c), d) dark fields revealing different parts of the same particle
335
TEM characterization of textured silicon heterojunction solar cells A. Hessler-Wyser1, C. Monachon1, S. Olibet2 and C. Ballif2 1. Interdisciplinary Centre for Electron Microscopy, Ecole Polytechnique Fédérale de Lausanne, 1015 Lausanne, Switzerland 2. PV-LAB, Institute of Microtechnology, University of Neuchâtel, 2000 Neuchâtel, Switzerland [email protected] Keywords: Heterojunction, thin films, HRTEM
Increasing the efficiency of crystalline silicon (c-Si) solar cells requires the reduction of both bulk and interface recombination. Even if bulk recombination is almost suppressed, the symmetry of the crystal lattice is disturbed at the surface and hence, due in particular to non-saturated bonds (dangling bonds), a large density of defects exists. Thus, in this case, the free-carrier lifetimes are no longer limited by the quality of the bulk c-Si, but by its surface. To keep the recombination losses at the c-Si surface at minimal levels, the surface must be electronically well passivated. An efficient way to obtain passivation is to use low temperature grown (typically 200°C) hydrogenated amorphous silicon (a-Si:H) [1]. In the case of photovoltaic applications, the passivation of both c-Si wafer surfaces (i.e., the emitter and the rear surface) is of crucial importance for good performances. In this work, the 3-7 nm a-Si:H based passivation layers of the device are grown by VHF-PECVD in a single chamber. The solar cells consist of a multilayered structure: Al back contact / DC-sputtered ITO (Indium Tin Oxyde) / n/i a-Si:H back surface field (BSF) / n-type c-Si substrate with a resistivity of 1-3 Ωcm / intrinsic a-Si:H / i/p a-Si:H emitter / and a front contact made out of DC-sputtered ITO via a shadow mask to define the cells (diameter = 4.5 mm). Such devices are called heterojunction (HJ) silicon solar cells. Surface recombination losses are a major concern for all c-Si solar cells. In particular, mastering of HJ emitter and back surface field formation on textured c-Si is crucial for high-performance HJ solar cells. High Resolution Transmission Electron Microscopy (HRTEM) is necessary to identify the key microstructural features of the aSi:H/c-Si interface, and TEM micrographs of HJ interfaces on flat and textured highperformance devices are shown for the first time and discussed with respect to the resulting solar cell electrical performances. TEM micrographs of our flat high-efficiency HJs show abrupt c-Si/a-Si:H/μc-Si:H interfaces for emitter and BSF formation. Whereas on the pyramidal facets of the textured substrate the growth is identical to the flat substrate interface, we observed unexpected epitaxial growth at the bottom of the pyramid valleys. We have identified these local epitaxial domains as an efficient surface recombination path, and by consequence, as responsible for the observed decreased VOC on textured HJ cells. When minimizing the density of epitaxial domains at the c-Si/a-Si:H interface by
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 335–336, DOI: 10.1007/978-3-540-85226-1_168, © Springer-Verlag Berlin Heidelberg 2008
336
adapting the deposition conditions, a solar cell VOC of 660 mV is obtained. An additional modification of the textured c-Si surface morphology leads to VOCs as high as 700 mV. 1.
J. I. Pankove and M. L. Tarng, Appl. Phys. Lett. 34, (1979),156.
Figure 1. HR-TEM micrograph of a flat Si HJ solar cell emitter consisting (from left to right) of c-Si / intrinsic a-Si:H / p+ a-Si:H/μc-Si:H layer. (The complete device includes a stack intrinsic a-Si:H / n+ a-Si:H/μc-Si:H layer stack for the back surface.) This structure yields HJ devices with VOCs of up to 710 mV and efficiencies up to 19.1%.
Figure 2. TEM and HR-TEM micrographs of a textured Si HJ solar cell emitter consisting of c-Si / intrinsic a-Si:H / p+ a-Si:H/μc-Si:H layer. In comparison with Fig. 1, one can observe epitaxy of the a-Si:H-based passivation layer located at the bottom of the pyramid valleys. Minimization of the density of such local epitaxial domains leads to Si HJ solar cell VOCs over 700 mV. Therefore, we identify such local epitaxial domains as unsatisfactory passivated spots at the c-Si/a-Si:H interface.
337
Investigation of the change in the microstructure of thin p-type Bi-Sb-Te thermoelectric films after heat treatment F. Heyroth1, M. Schade1, K. Rothe1, H.S. Leipner1 and M. Stordeur2 1. Interdisziplinäres Zentrum für Materialwissenschaften, Martin-Luther-Universität, 06099 Halle, Germany 2. angaris GmbH, Heinrich-Damerow-Str. 1, 06120 Halle, Germany [email protected] Keywords: thermoelectric film, LVSEM, EDX
Thermoelectric devices utilizing the Peltier and the Seebeck effect have been widely used for cooling and power generation applications in the last decades. Typically they are built from bulk materials. The energy conversion efficiency of such devices depends on the thermoelectric figure-of-merit (z⋅T) of the thermoelectric materials. In spite of numerous works to improve the z⋅T values of thermoelectric materials - which are dependent on the Seebeck coefficient S, the electrical conductivity σ, and the thermal conductivity κ (z = S²⋅σ / κ) - only a value around unity could be reached for bulk thermoelectric materials at room temperature. However, for low dimensional nanostructures, such as nanowires or superlattices, it has been predicted that the z⋅T values can be enhanced significantly compared to bulk materials due to quantum-confinement effects [1]. Beside this effect the progressive miniaturization requires thin thermoelectric films with Seebeck coefficients and electrical conductivities comparable to the bulk materials. Our films of the thermoelectric effective p-type compound semiconductor (Bi0 15Sb0 85)2Te3 were prepared by sputter-deposition. After heating of the as-deposited films and afterwards cooling, a distinct increase of the electrical conductivity σ can be observed. Measurements of the Seebeck and the Hall coefficient established that the increase of the electrical conductivity is not connected with an expected decrease of the Seebeck coefficient, because the charge carrier density is reduced but at the same time the hole mobility is increasing. The increase of the electrical conductivity at nearly unchanged Seebeck coefficient can be exploited for the enhancement of the film power factor (S²⋅σ). For the enlightenment of the changes in the film corresponding analytical investigations of the microstructure by XRD, EDX, and LVSEM were done. They show that, besides a grain growth in the polycrystalline films, a Te-rich phase appears after the heat treatment (cp. Figure 1). Also a generation of pores can be observed. The study of the crystalline nanostructure will be completed by EBSD and TEM investigations of the films. 1.
R. Venkatasubramanian, E. Siivola, T. Colpitts and B. O'Quinn, Nature 413 (2001) p. 597
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 337–338, DOI: 10.1007/978-3-540-85226-1_169, © Springer-Verlag Berlin Heidelberg 2008
338
Figure 1. Left: Comparison between SEM micrographs of the cross section surface of the thermoelectric film (a) before and (b) after thermal treatment. Right: Corresponding EDX-line scans (integrated EDX mappings) along the cross section using a polished sample.
339
EM study on forming Inorganic film with Periodically Organized Mesopores upon Polymer film Huang Wenqing1,2, Zhang Ying2, Yang Fang1, Zhaoxi2, Yang Wantai1 1. College of Material Science and Technology, Beijing University of Chemical Technology, Beijing 100029, China 2. Beijing Research Institute of Chemical Industry, SINOPEC. Beijing 100013, China [email protected] Keywords: Hybrid Thin Film, MCM-41, BOPP, PE
The potential use of nano-structured porous materials is currently recognized in advanced domains in materials chemistry, such as optical devices, photo-catalysis, catalysts, adsorption and sensors. The chemical nature and the morphology of the porous network can be accessed by XRD, IR, RAMAN, MAS-NMR, BET, SEM and HRTEM, which help us to make a better understanding of the nanocsale structure– property relationships and to control hybrid interfaces. [1] Here, we present a synthetic approach to produce Mesoporous materials containing designed nanoporosity on surface of polymer film after hydrophilic modification by confined photo-catalytic oxidation method. We use SEM to study the surface morphology and the thickness of the nanoporous film, and TEM to study the array of nanopores. In this work, a new synthesis method was studied to form a silica thin film with periodically organized nanopores upon polymer film. The UV irradiation system was used to make a modified polymer surface with high hydrophilicity[2]. Where, firstly, BOPP or PE films were cleaned with deionized water and acetone, and then predetermined amount of persulfate salt aqueous solution was deposited on the bottom film with a micro-syringe; a top layer transparent to UV light covered this solution and the drop of solution was spread into an even and very thin liquid layer. UV irradiation intensity is set at 8800uw/cm2, and irradiation time is controlled within 100s; then immersed the modified surface into water for 15hr. A MCM-41 sol-gel was spread to the treated surface by spin-coating method, and condensing reaction was conducted in 30min under acidic condition with triblock copolymer surfactant at room temperature. The surface morphology and the thickness of the inorganic film was showed respectively in Fig.1 and Fig.2. The thickness of the film range from 100nm to 2 micron can be controlled by spin coating speed and sol-gel concentration. TEM picture (Fig.3) showed the parallel pores and regular array of silica film after calcination. The diameter of the parallel pores is about 3 to 5 nm which is evidenced by Nitrogen Physisorption. 1. 2.
Clément Sanchez, Cédric Boissière, Chem.Mater. 20(2008), p.682-737. 2. P. Yang, J. Y. Deng, W. T. Yang, Polymer 44(2003), p.7157-7164.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 339–340, DOI: 10.1007/978-3-540-85226-1_170, © Springer-Verlag Berlin Heidelberg 2008
340
Figure 1. Surface morphology of inorganic fillm by SEM
Figure 2. Cross-section morphology of inorganic film upon polymer film by SEM
0.2 µm
Figure 3. TEM morphology of the powder after inorganic film calcination
50 nm
341
Nanointerface analysis of hard coatings deposited by IBAD D. Kakas1, B. Skoric1, A. Miletic1 and L. Kovacevic1 1. FTN – Centre for Surface Engineering and Nanotechnology, Trg D. Obradovica 6, 21000 Novi Sad, Serbia [email protected] Keywords: nanointerface, IBAD, cross section polisher
In this research hard TiN coatings were deposited onto previously carburized steel substrates (0.165%C, 0.2%Si, 1.2%Mn and 1%Cr). In order to sustain substrate properties obtained during heat treatment, hard coatings should be deposited at very low temperatures (up to 120°C). Special attention has been given to improving adhesion, which usually presents a problem when using low temperature deposition. Ion Beam Assisted Deposition offers a solution for this problem. However, IBAD alone is not enough since the main influence on adhesion has the interface between coating and substrate [1,2]. Ion Beam Mixing (IBM) has been used in order to acquire nanointerface between hard TiN coating and steel substrate. Using Ion Beam Mixing one can achieve intensive mixing of the atoms of a substrate with the atoms of a deposited coating. The thickness of the nano interlayer can easily be regulated by correction of parameters such as evaporation rate, energy of additional bombardment, atom to ion ration, incident angle etc. [3]. In this research nanointerface thickness was varied between 10 and 60 nm and its influence on coating adhesion was analysed. Adhesion of the coatings was characterized using scratch test equipment ST 2000. A diamond prism was used during the measurements. Damaged area was inspected using scanning force microscope. Micrograph of the scratch channel at the maximum load (100N) reveals that effects of delamination are not visible on the sides yet only at the end of the channel (Figure 1). Obtained results indicate very high adhesion. Our earlier investigations [2] show that other authors report much lower adhesion of coatings deposited at low temperatures. The presence of the nanointerface plays highly important role on excellent adhesion. This was confirmed using EDX analysis at the end of the scratch channel (Figure 1). Results of the EDX analysis are presented in the Table I. Spectrum 1 obtained at the place where coating delamination appeared shows that there is a 5.57 % of Ti in the surface of the base material. This means that coating delamination occurred across the nanointerface which was produced using IBM process. One can easily see that there are very small differences in composition in spectra 2, 3 and 4. It can be concluded that moving of diamond prism even at the load of 100 N didn’t change surface quality of TiN coating. In order to acquire the image of the nanointerface, samples were prepared using the Cross Section Polisher and inspected with HRSEM (JEOL JSM-7001F). The images were acquired at the JEOL (Europe) SAS Application Centre. Figure 2 shows the cross section of nanointerface.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 341–342, DOI: 10.1007/978-3-540-85226-1_171, © Springer-Verlag Berlin Heidelberg 2008
342
Figure 1. Micrograph of the hard the scratch channel is presented in the left, detail of delaminated area is presented in the right of the figure. Table I. Chemical composition at the end of the scratch channel (weight %) Spectrum
N
Ti
Cr
Mn
Fe
1 2 3 4
0.00 20.51 18.03 18.30
5.57 31.85 35.37 43.20
1.02 0.55 0.63 0.49
1.35 0.75 0.60 0.52
91.58 45.08 44.08 36.15
Figure 2. Micrograph of the hard TiN coating is presented in the left, high-resolution micrograph of a cross section of the nanointerface is presented in the right of the figure. Results of this investigation indicate a possibility of a new field of application of hard coatings such as deposition onto carburized steel substrates. Steel substrate provides high mechanical properties and TiN coating provides high wear resistance. 1. 2. 3. 4.
W. Ensinger, A. Schröer and G.K. Wolf, Surface & Coatings Technology 51, (1992), p. 217. D. Kakas, B. Skoric, T. Novakov, A. Miletic and L. Kovacevic, 10th International Conference on Tribology, Serbiatrib ’07 (2007), p. 71. B. Skoric, D. Kakas, M. Rakita, N. Bibic and D. Perusko, Vacuum 76, (2004), p. 169. This project was financially supported by the Ministry of Science and Environmental Protection of the Republic of Serbia.
343
Transrotational crystals growing in amorphous Cu-Te film V.Yu. Kolosov, A.V. Kozhin, L.M. Veretennikov, C.L. Schwamm Physics Dept. Ural State Economic University, 8Marta 62, Ekaterinburg, 620219 Russia [email protected] Keywords: bend contours, internal crystal lattice bending, Cu-Te amorphous condensates
Crystallization in amorphous films often results in strong internal lattice bending: TEM reveals regular rotation of initial lattice orientation across the growing microcrystals [1]. According to electron diffraction data our deposits prepared by vacuum evaporation of Te layer upon Cu layer are initially amorphous in wide range of thickness and composition. Te crystals growing later in these films carry regular bend contour patterns on the TEM images useful [2] for careful analysis of lattice orientations and lattice bending. Crystallization was either spontaneous or initiated by the electron beam illumination. The crystals of hexagonal Te were formed more or less elongated (normally to [001]) with dominant orientations for the crystal centers <010> or <120>, Figure 1 (some grains with these orientations are marked). Such orientations correspond to most dense lattice planes lying almost parallel the surface (also parallel film plane). Bend contour technique was used to measure the magnitude of internal lattice bending (i.e. rotation of the lattice orientation) about two mutually perpendicular directions: around [001] and around its normal. Internal lattice bending around [001] is almost 4 times higher and is doubling (from 85 to 192 degrees per micrometer) upon film thickness reducing by half (from 40 nm to 22 nm), Figure 2. At the same time internal lattice bending around normal to [001] is increasing four times: from 12 to 50 and from 11 to 44 degrees per micrometer for orientations <010> and <120> correspondingly (in the central crystal areas where nucleation takes place). In addition the decrease of film thickness results in increase of aspect ratio. Anisotropy of internal lattice bending is caused by the character of chemical bonding (the covalent coupling of atoms in spirals lying along [001], and Van der Waals bonds between these spirals). Lattice orientation of the nucleus has less pronounced effect for a lattice bending (Figure 2). Qualitative estimates: the increase of Cu content rises internal lattice bending and reduces aspect ratio of the elongated grains, Figure 3. Often the total continuous rotation of the lattice orientation (corresponding to elastic bending) in the isolated crystals exceeds 180 degrees, Figure 4. Such large regular lattice misorientations (also published for other substances) unambiguously testify to the fact of internal (lattice) nature of the bending and cannot be caused by bending of a crystal as a whole body (for 180 degrees opposite corners of thin bent crystal should be nontransparent for electron beam). Thus the studied Te crystals can be associated with “transrotational” crystals [1]. 1. 2.
V.Yu. Kolosov and A. R. Tholen, Acta Mat. 48 (2000) p. 1829–1840. V.Yu. Kolosov, Proc. XII ICEM, ed. L. Peachey & D. Williams, (Seattle) 1 (1990) p. 574575.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 343–344, DOI: 10.1007/978-3-540-85226-1_172, © Springer-Verlag Berlin Heidelberg 2008
344
Figure 1. Micrographs of Te crystals with dominant orientations (marked for some grains by squares and circles) grown in areas of different film thickness (a – 38nm, b – 30nm, c – 22nm) and SAD (d)
Figure 2. Dependence of internal lattice bending in Te crystals upon the film thickness, measured for the grains from the upper Figure 1.
a
b
Figure 4. Te crystal with total lattice misorientation above 180˚ (from A to D). Internal lattice bending ~ 120˚/μm. ZAPs corresponding to <010> are marked with triangles. c
Figure 3. Te crystals in film areas with different Cu concentration (a – 22%, b – 20%, c – 18%). Aspect ratio goes down as the Cu content increases.
345
TEM investigation of sputtered indium oxide layers on silicon substrate for gas sensors Th. Kups1, I. Hotovy2 and L. Spieß1 1. Institute of Micro- and Nanotechnologies, Materials of Electronics, Ilmenau University of Technology, P.O. Box 100565, 98684 Ilmenau, Germany 2. Department of Microelectronics, Faculty of Electrical Engineering and Information Technology, Slovak University of Technology, Ilkovičova 3, 812 19 Bratislava, Slovakia thomas [email protected] Keywords: In2O3, PVD, HRTEM
Indium oxide (In2O3) has recently attracted much interest as a material for transparent electrodes in electronic devices such as liquid crystal displays [1], solar cells [2], as a barrier layer in tunnel junctions [3], as sensing material in gas sensors e.g. for ozone [4] and in nanowire technology [5]. Two crystal structures have been reported for In2O3: body-centered cubic (bcc, Ia3, a = 1.0118 nm) and rhombohedral (rh, R-3c, a = 0.5478 nm and c = 1.451 nm) [6]. In the case of bcc-In2O3, the physical and optical properties are well known [1-4], whereas for rh-In2O3, to the best of our knowledge, no information is available. Common deposition methods of In2O3 films and nanostructured layers are evaporation [7], magnetron sputtering [8] and Sol-Gel [9] processing. These deposition processes usually lead to the growth of In2O3 with a poly- or single crystalline bcc structure independent of the used substrate [10]. In this work magnetron sputtering technique will be used to form indium oxide layers and cross section high resolution transmission electron microscopy (HRTEM) for investigation of the crystal structure. Nanoscaled In2O3 films were deposited by dc reactive magnetron sputtering from a In target (76.2 mm in diameter, thickness of 3 mm and 99.99% pure) in a gas mixture of O2 and Ar. The distance between the target and substrate was approximately 75 mm. The apparatus was evacuated to a pressure below 5x10-4 Pa before deposition. A sputtering power of 75 W was used. Both the inert argon flow and reactive oxygen flow were controlled by mass flow controllers. The flow of oxygen in the reactive mixture O2-Ar was changed in the range of 40-80 sccm. The thicknesses of the resulting layers were in the range of 40-80 nm which were prepared onto unheated silicon substrates. Figure 1 shows the comparison of different layers sputtered at different growth parameters (Fig 1a, b: O2 flow 40 sccm compared to 80 sccm in Fig. 1c, d). The HRTEM images show different crystalline structures sizes and shape. While in the low oxygen flow case (Figs. 1a and b) the size of the crystallites is in the range of >20 nm and so in the FFT spots a clearly visible, for the higher oxygen case the particle size decreased into the range of ~10 nm and the polycrystalline structure was increased. For both samples the majority of reflexes correspond to rhombohedral In2O3 whereas some single reflexes could associate with cubic phase!
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 345–346, DOI: 10.1007/978-3-540-85226-1_173, © Springer-Verlag Berlin Heidelberg 2008
346
d b
Figure 1. (HR)TEM images of In2O3 layers formed by using low (a and b) and high (c and d) oxygen flow while reactive magnetron sputtering. The differences in crystallinity presented in the FFT inset in b and d show smaller particle sizes for the high oxygen flow case. The majority of the FFT reflexes correspond to the rhombohedral In2O3 phase. 1.
C. Falcony, J. R. Kirtley, D. J. Dimaria, T. P. Ma, and T. C. Chen, J. Appl. Phys. 58, 3556 (1985) 2. C. G. Granqvist, Appl. Phys. A 57, 19 (1993) 3. S. Kasiviswanathan and G. Rangarajan, J. Appl. Phys. 75, 2572 (1994) 4. M. Bender, N. Katsarakis, E. Gagaoudakis, E. Hourdakis, E. Douloufakis, V. Cimalla and G. Kiriakidis, J. Appl. Phys. 90, 5382 (2001) 5. Ch. Li, D. H. Zhang, B. Lei, S. Han, X. L. Liu, and Ch. W. Zhou, J. Phys. Chenm. B 107, 12451 (2003) 6. ICDD PDF-2 Data base, JCPDS-Int. Center for Diffraction Data, Pennsylvania, USA (2006). 7. C. A. Pan, and T. P. Ma, Appl. Phys. Lett. 37, 163 (1980). 8. S. Kasiviswanathan and G. Rangarajan, J. Appl. Phys. 75, 2572 (1993). 9. H. Imai, A. Tominaga, H. Hirashima, M. Toki, and N. Asakuma, J. Appl. Phys. 85, 203 (1998). 10. Ch. Y. Wang, V. Cimalla, H. Romanus, Th. Kups, G. Ecke, Th. Stauden, M. Ali, V. Lebedev, J. Pezoldt, and O. Ambacher, Thin Solid Films 515 (2007) 6611–6614 11. This project is supported by the German Academic Exchange Services (DAAD) within project D/06/07398
347
Microstructure of Sr4Ru2O9 thin films and Bi3.25La0.75Ti3O12/Sr4Ru2O9 bilayers R. Chmielowski1,2, V. Madigou1, M. Blicharski2, Ch. Leroux1 1. IM2NP (UMR-CNRS 6242), South University Toulon-Var (USTV), Bat.R , B.P.20132, 83957 La Garde Cedex, France 2. AGH - University of Science and Technology, Al. Mickiewicza 30, 30-059 Kraków, Poland [email protected] Keywords: Sr4Ru2O9, pulsed laser deposition, oxide electrode
It has been reported that using oxide bottom electrodes reduces the fatigue phenomenon in ferroelectric random access memories (FeRAM). For that aim, strontium ruthenate SrRuO3 was already used as bottom oxide electrode for ferroelectric thin films [1], but compounds with less ruthenium are more interesting from the economical and environmental point of view. We elaborate Sr4Ru2O9 thin films and bilayers Bi3 25La0 75Ti3O12 /Sr4Ru2O9 by pulsed laser deposition. Sr4Ru2O9 compound differs from the other strontium ruthenates. It has a hexagonal perovskite structure, contains pentavalent ruthenium atoms, with octahedral sharing faces, thus building dimmers Ru2O9 [2]. All the other strontium ruthenates belong to the Ruddlesden Poppers homologous series, Srn+1RunO3n+1 (Sr2RuO4 corresponds to n=1 and SrRuO3 to n=∞). The common features of these compounds are an orthorhombic structure, tetravalent ruthenium atoms, and an octahedral surrounding by oxygen of ruthenium atoms. The films were grown by pulsed laser deposition on Si [100] substrate, using a Sr2RuO4 target with an excimer laser (KrF λ=248 mm, COMPex 301, Lambda Physik). The laser beam had a fixed size of 2mm x 5 mm and the fluence of the laser on the target was 1.5 Jcm-2. The substrate was heated up to 700°C and the films were deposited in two different oxygen pressures, 50 10-3 Torr and 300 10-3 Torr [3]. The thin films and the targets were characterized by X-ray diffraction; in order to identify the strontium ruthenate phases. The surface morphology of the target and the thin films was observed with a JEOL JSM-6320F high resolution scanning microscope. A Tecnai G2 transmission electron microscope, operating at 200 kV with a LaB6 filament, equipped with a 1k x 1k Slow Scan CCD camera, was used for microstructural characterizations. All electron diffraction patterns obtained with various zone axes were indexed in the Sr4Ru2O9 hexagonal structure and each time, diffuse streaks parallel to a* or b*, were present (Figure 1). The occurrence of forbidden spots could be explained by an ordering of Ru atoms. In the case of Sr4Ru2O9 films, transmission electron microscopy revealed, on cross section samples, the existence of a supplementary strontium ruthenate phase, in form of nanograins, layered on top of the Sr4Ru2O9 columnar grains, for all the thin films deposited with 50 mTorr oxygen pressure in the deposition chamber. This is at the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 347–348, DOI: 10.1007/978-3-540-85226-1_174, © Springer-Verlag Berlin Heidelberg 2008
348
origin of the intermediaire layer observed the ferroelectric film and the oxide electrode. For thin films Bi3 25La0 75Ti3O12 /Sr4Ru2O9, this layer is single phase and has a SrTiO3 structure. 1. 2. 3.
H.N.Lee, D.Hesse, N.Zakharov,U.Gösele, Science 296 (2002), 2006 C.Dussarat, J;Fompeyrine, J.Darriet, Eur.J. Solid State Inorg. Chem. 32, (1995), 3 R. Chmielowski, V. Madigou, Ph. Ferrandis, R. Zalecki, M. Blicharski, Ch. Leroux, Thin Solid Films, 515 (2007), 6314
Figure 1. Cross sectional view of Bi3 25La0 75Ti3O12 /Sr4Ru2O9 Diffraction patterns taken on the Sr4Ru2O9 films, corresponding to [010] (a) and to [201] zone axes (b).
BLT Intermediate layer Sr4Ru2O9 100 nm
Figure 2. Cross sectional view of a Bi3 25La0 75Ti3O12 /Sr4Ru2O9 bilayer, showing the occurrence of a well crystallized intermediate layer.
349
Analysis of the LSM/YSZ interface on microand nano-scale by SEM, FIB/SEM and (S)TEM Yi-lin Liu, Luise Theil Kuhn and Jacob R. Bowen Fuel Cells & Solid State Chemistry Department Risø National Laboratory for Sustainable Energy, Technical University of Denmark DK-4000 Roskilde, Denmark [email protected] Keywords: interface, nano-structure, FIB/SEM, (S)TEM
8 mol% Y2O3-stabilized ZrO2 (8YSZ) and lanthanum strontium manganite (LSM) are well developed materials for electrolyte and cathode, respectively, in solid oxide fuel cells (SOFCs). Thermodynamically the 8YSZ/LSM interface is not stable and solid state reactions will result in formation of zirconates (La2Zr2O7, SrZrO3) which are electrically insulating phases. For cells operated at 1000˚C, zirconates were found covering large areas of the interface: this was readily characterized by XRD, SEM, TEM and identified as a degradation mechanism in SOFC [1,2]. However, the newly developed SOFCs are operated at much lower temperatures (700-800oC). Due to the slow reaction kinetics, the zirconate formation is localized and its growth is limited. In this case, identification of microstructural degradation has become a great challenge. This paper presents how such an interface has been studied by FEGSEM, FIB and (S)TEM combined with EDS from the micro- to nanometre scales. The interface sample used in this work was taken from a cell that has been tested at 750˚C for 1500h. The cathode was removed by HCl etching (LSM dissolves quickly whereas 8YSZ and La2Zr2O7 are not affected in HCl) and then the electrolyte surface was analyzed using a Zeiss Supra FEGSEM. A low accelerating voltage of ~2 kV was used which allowed direct imaging of the 8YSZ surface without carbon coating. The contact points left over by (dissolved) LSM grains (a few hundred nanometre) appear as craters, and many nanoparticles are found in association with these craters (Figure 1). To identify these nanoparticles lining the craters, a site-specific TEM lamella was made using a Zeiss 1540XB CrossBeam microscope. Prior to the FIB milling several protective layers of W were deposited on the area where the lamella later was extracted. Firstly, to avoid excessive Ga ion damage to the nanoparticles a 60 nm thick W layer was locally electron beam deposited using the in-situ chemical vapour deposition gas injection system (GIS). Subsequently, the Ga ion beam was used with the GIS to deposit successively thicker W protection layers with increasing Ga ion beam probe currents. After building up a 1.5 µm thick protective layer the lamella was extracted using the standard in-situ TEM lamella preparation technique. The lamella dimension was 1 x 30 x 8 µm3 (thickness, length and depth, respectively) prior to mounting on a Cu Omniprobe™ TEM sample holder. Final thinning was performed in a 24 x 2 µm window until the region with the crater surfaces was approximately 50 nm thick suitable for high resolution TEM, STEM and EDS investigation (Figure 2).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 349–350, DOI: 10.1007/978-3-540-85226-1_175, © Springer-Verlag Berlin Heidelberg 2008
350
The (S)TEM analysis was performed using a 300kV Jeol 3000F TEM equipped with a Gatan Imaging Filter (GIF), a STEM unit and an Oxford Inca EDS system. The craters were studied in normal TEM and in STEM mode, and their chemical composition and environment were analysed by site-specific nanobeam EDS with an average electron beam diameter of 10 nm. Nanoparticles with sizes in the range 3-20 nm (see Figure 3) were only observed in the crater regions confirming the SEM studies. EDS analysis was performed in several crater regions and also at the crater environment to detect any changes in chemical composition. The EDS analysis of nanoparticles showed that there are clear observations of La- and Sr-phases further confirming the hypothesis that the nanoparticles are a result of the cathode degradation and are closely connected with the contact points of the LSM grains. The TEM and EDS studies were supplemented by STEM imaging where the enhanced contrast favoured imaging of the crater rims and the nanoparticles. 1. 2.
E. Ivers-Tiffee, A. Weber, K. Schmid and V. Krebs, Solid State Ionics, 174 (2004) p. 223. A. Mitterdorfer and L.J. Gauckler, Solid State Ionics, 111(1998) p. 185.
Figure 1. SEM image showing LSM craters and nano-particles on the 8YSZ electrolyte surface.
Figure 2. SEM image of the TEM lamella after extracted and thinned.
Figure 3. TEM image showing the cross section of a crater region with nanoparticles. The light and dark region to the left of the diagonal is the protective layer of W and the dark contrast is caused by implanted Ga. Only a few % of Ga was detected in the nanoparticles, so we assume that they were not affected by the Ga-ion beam. The circles indicate some of the larger nanoparticles at the electrolyte (dark contrast to the right) interface.
351
ESI and HRTEM of chemical solution deposited (CSD) YBa2Cu3O7-δ coated conductors L. Molina1, T. Thersleff2, B. Rellinghaus2, B. Holzapfel2, O. Eibl1 1. Institut für Angewandte Physik, Eberhard-Karls Universität Tübingen Auf der Morgenstelle 10, D-72076, Tübingen, Germany 2. IFW Dresden, P.O. Box 270116, D-01171, Dresden, Germany leopoldo [email protected] Keywords: thin films, interfaces, coated conductors
Coated conductors are currently of great interest for technological applications which involve transportation of large currents. TEM Sample preparation techniques and CTEM analysis are presented in other papers at this conference. Control of the stoichiometry of CSD prepared films is a key issue for coated conductor technology. Performance limiting secondary phases have to be eliminate or minimized during film deposition. Thus, a reliable nano-scaled chemical analysis is crucial for coated conductor fabrication. The chemical composition and distribution within YBCO-coated conductor samples of Ni5at%W(substrate)/La2Zr2O7(CSD)/CeO2(CSD)/YBCO(CSD) layer architecture was studied by energy-filtered TEM (ESI) in a Zeiss 912 OMEGA operating at 120 kV. By electron spectroscopic imaging (ESI), elemental maps with high lateral resolution of YBCO-coated conductor samples in cross-section were obtained. Fig.1 shows an RGB overlay of Ce, Ba, Y and La elemental maps. The used ionization edges are outlined in table 1. The Ni substrate, the La2Zr2O7 and the YBCO thin film appear in strong contrast. An intermediate layer is found between the Ni and the LZO. Two YBCO layers were deposted for this sample by CSD and these layers and their interface are clearly imaged, e.g. 100 nm Yttria secondary phases (blue in fig. 1) which were identified by energy dispersive X-ray microanalysis in the TEM. Understanding the Ni/oxide interface is of crucial importance for the deposition of biaxially textured LZO buffer layers. The small lattice parameters of the Ni substrate requires a point resolution of significantly better than 0.2 nm. Therefore, the crosssection sample of fig.1 was analysed in a FEI-TITAN 300 kV transmission electron microscope equipped with a Cs corrector yielding a point resolution of better than 0.1 nm. Fig.2 shows a cross-section of a Ni/oxide interface. 1.
Molina L, Knoth K, Engel S, Holzapfel B, Eibl O 2006 Supercond. Sci. Technol. 19 12001208
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 351–352, DOI: 10.1007/978-3-540-85226-1_176, © Springer-Verlag Berlin Heidelberg 2008
352
Figure 1. ESI chemical maps of a full YBCO-coated conductor sample. R(Ce)G(Ba)B(Y) overlay image and ESI R(Ce)G(Ba)B(La) overlay image Table 1. a.) Ionization edges used. Ce (N 4,5)
La (N 4,5)
La (M 4,5)
Ba (N 4,5)
(eV)
(eV)
(eV)
(eV)
ΔE1
76
76
127
60
ΔE2
102
95
149
80
ΔE3
137
118
184
111
Edges
Pre-edge 1 Pre-edge 2 Post-edge
Figure 2. HRTEM of the Ni /oxide interface. Lattice spacing in Ni is 0.2 nm.
353
CTEM diffraction contrast of biaxially-textured La2Zr2O7 buffer layers on nickel substrates L. Molina1, S. Engel2, B. Holzapfel2, O. Eibl1 1. Institut für Angewandte Physik, Eberhard-Karls Universität Tübingen Auf der Morgenstelle 10, D-72076, Tübingen, Germany 2. IFW Dresden, P.O. Box 270116, D-01171, Dresden, Germany leopoldo [email protected] Keywords: thin films, interfaces, coated conductors
Chemically deposited La2Zr2O7 (LZO) buffer layers are of crucial importance for YBCO-coated conductor fabrication. They transfer the texture from a highly biaxially textured nickel tungsten substrate to the final YBCO superconducting layer and act as nickel diffusion barriers. The misfit of LZO with respect to the nickel tungsten substrate is 7.6% (compressive). LZO films were grown by Chemical Solution Deposition (CSD) and were annealed at temperatures between 900°C and 1000°C [1]. The films are highly biaxially textured as suggested by the XRD pole figures shown in figure 1 [2]. Due to the XRD pole figures an epitaxial growth of LZO is claimed in the literature, which was the motivation for this investigation. Conventional TEM two-beam diffraction contrast imaging is sensitive to small misorientation of grains and allows to image small-angle grain boundary networks present in the LZO thin films. Carefully tilting the sample under two-beam conditions reveals grains of 100-200 nm in size that are slightly titled with respect to each other and to the underlying Ni grain in the substrate, (figure 3 plan-view LZO sample). Dark areas are grains that are in a strong diffraction condition. The contrast of these images are particularly sensitive to the out-of-plane tilt of the crystallites. Figure 2 shows a similar sample prepared as cross-section and LZO grains of 100-200 nm can be identified. The average Ni substrate grain size is 40 μm and the LZO grain size is 100200 nm, therefore epitaxial growth of LZO on Ni does not occur . Figure 4 shows a dark-field image at the Ni-LZO interface under two-beam diffraction conditions using the g(400) reflection of LZO. Bright areas show LZO grains that are in a strong diffraction contrast condition denoted in the figure as grain 1 to 5. Also observed in the images is the strong contrast from the nanovoids present in the films [3]. At the Ni /LZO interface a roughness with a wavelength of 60 nm and an amplitude of 10 nm is found. LZO grain size was beyond 100 nm and agrees with plan view results. The LZO grains are shown to extend over the full film thickness. The tilting of the LZO grains and the roughness at the interface contribute to strain relief in the LZO film. 1. 2.
Molina L, Engel S, Knoth K, Hühne R, Holzapfel B, Eibl O 2008 Journal of Physics: Conference Series 97 (2008) 012108 Molina L, Knoth K, Engel S, Holzapfel B, Eibl O 2006 Supercond. Sci. Technol. 19 12001208
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 353–354, DOI: 10.1007/978-3-540-85226-1_177, © Springer-Verlag Berlin Heidelberg 2008
354
Figure 1. (a-b) XRD pole figures. Figure 2. TEM bright-field images under two beam conditions of an LZO buffer layer sample in crosssection (a-c). Nano-voids 10-20 nm in size can be seen. (d-f) corresponding dark-field images. Note that all images are from the same sample area. The white arrow indicates a LZO grain.
Figure 3. TEM bright-field image tilt series of an LZO buffer layer sample in planview. Scale bar is 100 nm
Figure 4. Dark-field image under two beam conditions of an LZO buffer layer sample in cross-section. The horizontal white arrow indicates the interface. Vertical arrows show roughness at the interface.
355
TEM sample preparation of YBCO-coated conductors: conventional method and FIB L. Molina1, T. Thersleff2, C. Mickel2, S. Menzel2, B. Holzapfel2, O. Eibl1 1. Institut für Angewandte Physik, Eberhard-Karls Universität Tübingen Auf der Morgenstelle 10, D-72076, Tübingen, Germany 2. IFW Dresden, P.O. Box 270116, D-01171, Dresden, Germany leopoldo [email protected] Keywords: thin films, interfaces, coated conductors
YBa2Cu3O7-δ (YBCO)-coated conductors prepared by the chemical solution deposition process (CSD) are currently of great interest for industrial applications. A flexible nickel tungsten substrate is dip-coated in a buffer layer and a YBCO precursor solution. The resulting thin films systems have a high misfit. TEM sample preparation is challenging and is a fundamental issue for the characterization of YBCO-coated conductors. Conventional sample preparation involves gluing the sample of interest between oxide and silicon dummies followed by mechanical polishing and grinding [1]. Further thinned is done using Ar+ ions in a Baltec Res 100 ion milling machine operating at 4.5 kV and 3.5 mA with etching angles ranging from ±12° to ±6° for up to 30 hrs. The insitu lift-out focused ion beam (FIB) allows to prepare as TEM lamellas previously choosen sample areas. Figure 1 describes the preparation procedure. A Pt protection layer is deposited on top of the area of interest in the YBCO film. Trapezoid shaped cuts area made with a Ga-ion beam. The in-situ lift-out is done with a nanomanipulator. The sample is attached to a sample holder and further ion milled until reaching ~100 nm thickness. Samples prepared by this method are highly homogenous which makes them especially suitable for electron spectroscopic imaging (ESI) and HRTEM. 1.
Eyidi D, Eibl O 2002 Micron 33 499
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 355–356, DOI: 10.1007/978-3-540-85226-1_178, © Springer-Verlag Berlin Heidelberg 2008
356
Figure 1.- a.) Pt protection layer deposited on the area of interest on top of the YBCO film. Scale bar is 1 μm b.) Trapezoid shaped cuts made with the Ga-ion beam. Scale bar is 1 μm c.) In-situ lift out of the TEM lamella done with a nano-manipulator. Scale bar is 10 μm d.) Attachment of the TEM lamella to the half-grid sample holder Scale bar is 100 μm e.) Encircled area shows were the sample was attached. Scale bar is 100 μm f.) Overview of the polished final TEM lamella. Scale bar is 1 μm.
Figure 2.- a.) Zero-loss dark-field image of FIB prepared TEM lamella. b.) Zero-loss dark-field image of a conventionally prepared sample.
357
Nucleation and evolution of biepitaxial YBa2Cu3O7-δ thin film grown on SrTiO3 and MgO substrates H. Pettersson1, K. Cedergren2, D. Gustafsson2, R. Ciancio1, F. Lombardi2 and E. Olsson1 1. Dept. of Applied Physics, Chalmers University of Technology, Göteborg, Sweden 2. Dept. of Microtechnology and Nanoscience, Chalmers University of Technology, Göteborg, Sweden [email protected] Keywords: Nucleation, thin films, YBa2Cu3O7-δ, SrTiO3, MgO
The importance of the microstructure for the transport properties of grain boundaries in high-temperature superconducting YBa2Cu3O7-δ (YBCO) (e.g. SQUID-based devices) is well established. Basal-plane grain boundaries can be used as high-quality Josephson junctions [1,2]. In this work artificial grain boundaries (AGB) of (103)/(001) YBCO films produced by pulsed laser deposition (PLD) have been investigated, in order to obtain knowledge of the YBCO film nucleation and the subsequently grain boundary evolution. For this purpose ultra thin films (50 and 100 pulses) and full films have grown on two different substrate/template-layer combinations (110) MgO / (110) SrTiO3 (STO) and (110) STO / (110) CeO2 (CEO) respectively. The (103)/(001) YBCO biepitaxial artificial grain boundaries were obtained on substrates with a vicinal cut, in order to achieve pure (103) YBCO growth on top the STO regardless if STO is used as substrate or template-layer. The YBCO grow with (001) orientation and 45º in-plane rotation on the MgO and CEO. The microstructural investigation has been performed with scanning electron microscopy (SEM) using a Leo Ultra 55 FEG SEM. The transmission electron microscopy (TEM) investigation was carried out using a Philips CM 200 FEG and JEOL JEM 2100-F both operated at 200kV. The results show that the nucleation site (see Fig. 1) of the YBCO depends on the morphology of the substrate close to the step (See Fig. 2). Both (103) and (-103) YBCO are found at the YBCO/STO interface due to surface roughness, exposing both (100) and (010) facets. The nucleation of YBCO film and subsequently growth at the step edge, produced by the etching procedure, affects the grain boundary evolution. By growth of ultra thin YBCO films the nucleation sites of YBCO could be determined. 1. 2.
Granozio, F.M., et al., Structure and Properties of a Class of CeO2-based Biepitaxial YBa2Cu3O7-™ Josephson Junctions. Physical Review B, 2003. 67(18). Tafuri, F., et al., Microstructure and Josephson phenomenology in 45 degrees tilt and twist YBa2Cu3O7-™ artificial grain boundaries. Physical Review B, 1999. 59(17): p. 11523-11531.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 357–358, DOI: 10.1007/978-3-540-85226-1_179, © Springer-Verlag Berlin Heidelberg 2008
358
a)
(103) YBCO c)
b)
(001) YBCO (001) YBCO
(103) YBCO
(103) YBCO
(001) YBCO
d)
(001) YBCO
(103) YBCO
Figure 1. SEM micrographs of (103)/(001) YBCO films grown on STO substrates with a) 50 pulses, b) 100 pulses and c) full thickness, (-103) oriented YBCO growth is marked (red), and d) full thickness on MgO substrate
Figure 2. TEM micrograph of (103)/(001) YBCO films grown on MgO substrate.
359
An investigation of Al-Pb interfaces using probe-corrected high-resolution STEM Harald Rösner1, Sergei Lopatin2, Bert Freitag2 and Gerhard Wilde1 1. Westfälische Wilhelms-Universität Münster, Institut für Materialphysik, Wilhelm-Klemm-Str. 10, D-48149 Münster, Germany 2. FEI Company, Achtseweg Noord 5, 5600 KA Eindhoven, The Netherlands [email protected] Keywords: high-resolution STEM, probe Cs-corrector, misfit dislocation
Nanometre-sized Pb inclusions embedded in an Al host matrix serve as a model system for size-dependent melting studies [1-3]. For this purpose, an Al-Pb composite containing 1 at.% Pb was prepared by high-energy ball milling. Former TEM investigations revealed that the metal/metal interfaces were found to display a cube-on-cube orientation relationship with a large lattice mismatch of 22% with respect to the Al lattice [14]. The accommodation of the lattice misfit has remained a puzzle until quite recently due to Moiré contrasts that veiled a direct observation of the interface structure. Recently, this mismatch has been visualized by high-resolution TEM of uncovered Pb inclusions [4,5] displaying a hetero-interface with the Al matrix remaining on one side only. Such Pb particles were located in the amorphous edge area of the TEM specimen. In this study, partially embedded Pb inclusions located in the thicker part of the TEM foil, having hetero-interfaces on all lateral sides with the Al matrix, have been analyzed. For this purpose, high-resolution HAADF-STEM investigations have been carried out in a FEI Titan 80-300 (field-emission gun, super-twin lens, Cs= 1.2 mm, monochromator) operated at 300 kV and equipped with a CEOS Cs probe-corrector. The spherical aberration of the probe has been corrected down to the level of a few microns. Fourier-filtering was performed on the high-resolution micrograph using the Digital Micrograph Software Package (Version 3.7.4, Gatan). Circular masks with a diameter of 0.5 nm have been used for the Fourier-filtering in Figure 2. In Figure 1 two Pb inclusions embedded in an Al matrix are shown. The larger inclusion appears faceted but without a Moiré pattern. The smaller one has a spherical shape and a strong Moiré contrast. The insert in Figure 1 is the Fourier transform of the whole image. The Al and Pb reflections of the [011] zone axis confirm the cube-oncube orientation relationship. The observation of a partially encased faceted Pb inclusion in the thicker part of the TEM foil allows a direct comparison with the results of former studies [4,5] where the Pb inclusions investigated were located in the thinnest parts of the TEM foil. Here by use of high-resolution STEM imaging instead of HRTEM, one may discern that even in the thicker parts of the TEM foil the lattice misfit at the Al/Pb interface is localized in the form of interfacial dislocations. In the absence of a Moiré pattern, the faceted Pb inclusion shown in Figure 2 can be seen to display a semicoherent interface with the Al matrix. A misfit on about every fifth Al plane is observed; white lines indicating their positions have been added to guide the eye. In addition, the current observation provides the opportunity to learn more about the particle S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 359–360, DOI: 10.1007/978-3-540-85226-1_180, © Springer-Verlag Berlin Heidelberg 2008
360
shapes with respect to matrix strains [6]. Since most of the Pb inclusions in ball-milled Al-Pb composites exhibit curved non-faceted shapes, the question arises why in this case one of the Pb inclusions shows a faceted morphology. The answer may be found in the fact that this Pb inclusion was only partially embedded in the Al matrix without an overlapping Al layer above or underneath. As a result the strain relief is thought to be accomplished via these two ‘free’ surfaces by the high mobility of the Pb atoms [1]. In contrast, the fully embedded Pb inclusion nearby, displaying a curved morphology, is totally governed by strains of the heavily distorted Al matrix. A strain relief in the distorted Al matrix of ball-milled material achieved by annealing also led to a change in particle shapes [6]. Thus, faceted interfaces account for a lower total excess free energy of the nanoparticle and hence, a melting point increase. 1. 2. 3. 4. 5. 6. 7.
E. Johnson, H.H. Andersen, and U. Dahmen, Microsc. Res. Techniq. 64 (2004), p. 356. K. Chattopadhyay and R. Goswami, Prog. Mater. Sci. 42 (1997), p. 287. Q.S. Mei and K. Lu, Prog. Mater. Sci. 52 (2007), p. 1175. H. Rösner, J. Weissmüller, and G. Wilde, Phil. Mag. Lett. 86 (2006), p. 623. H. Rösner, B. Freitag, and G. Wilde, Phil. Mag. Lett. 87 (2007), p. 341. H. Rösner, P. Scheer, J. Weissmüller, and G. Wilde, Phil. Mag. Lett. 83 (2003), p. 511. The experiments have been performed during a FEI Demo at the Ernst-Ruska Centre in Jülich.
Figure 1. High-resolution HAADF-STEM micrograph showing two Pb inclusions embedded in an Al matrix projected along the [011] zone axis. The larger particle shows clear facets and no Moiré pattern. The smaller Pb inclusion appears spherically shaped and with a Moiré pattern due to the overlapping Al matrix. The inset shows the Fourier transform revealing the cube-on-cube orientation relationship between the two lattices.
Figure 2. Detail of Figure 1 showing the faceted Pb inclusion after Fourier-filtering. Masks were set around all reflections in order to remove the noise. The lattice mismatch is indicated by the white lines. No Moiré pattern is visible.
361
Spectrometric Full-Color Cathodoluminescence Electron Microscopy Study of Grain Boundaries of ZnO Varistor H. Saijo1, N. Daneu2, A. Recnik2, and M. Shiojiri3 1. School of Biology-Oriented Science and Technology, Kinki University, 930 Nishimitani, Kinokawa, Wakayama 649-6493, Japan 2. Jozef Stefan Institute, Jamova 39, SI-1001 Ljubljana, Slovenia 3. Prof. Emeritus of Kyoto Institute of Technology, 1-297 Emmyoji-Wakiyama, Ohyamazaki, Kyoto 618-0091, Japan (home) hirsaijo@waka kindai.ac.jp Keywords: cathodoluminescence, ZnO, varistor
Scanning electron microscopy (SEM) with cathodoluminescence (CL) detection can draw a map of electronic states and chemical bonding in the specimen. The energy of CL photons gives information of Band Gap of semiconductors or Highest Occupied Molecular Orbital (HOMO)-Lowest Unoccupied MO (LUMO) of organic materials. Our new spectrometric full-color CL microscope [1] obtains CL spectra of each observing point and draws full-color CL micrograph and SEM image of 512 x 512 pixels in 8 s. The block diagram of the system is shown in Fig. 1. Spatial resolution of CL micrographs is worse than that of SEM due to bulb-shape spread of incident electrons in solids. Delayed CL emission is another cause of poor resolution. Both result practical CL resolution around 100 nm. However, lower incident energy and slow image scan improve the resolution significantly, and in our system 25 nm resolution was verified with 6 kV beam and 40 s/frame. With this high resolution, we observed grain boundaries of ZnO varistor ceramics with 1 mol % of Bi2O3. The specimen also contains SnO2 from 0.1 to 10 mol %. The grain size of the ZnO decreased with increasing amount of SnO2. [2] However, electronic properties did not show significant difference with SnO2 concentration. We examined CL spectra of boundaries, surface and cutout plane of the ZnO grains as shown in Figs. 2 and 3. The cutout plane can be regarded as the inside bulk of the grain. The grain surfaces emit strong bluegreen CL, and the bulk emits weak or no luminescence. CL observation across the boundary revealed that several peaks appear and disappear depending on the position from the boundary. 500 nm peak appears first (Fig. 2-7), and then 510 nm peak rises if mouse-pointer moved slightly inward the grain. Then, 490 nm peak appears forming twin with 510 nm peak. Further inside shows various CL peaks as shown in Fig. 3-4 and 3-5. CL peaks between 490 and 510 nm observed across the boundary correspond to the layers with different composition, and all of them appear in every specimen of different SnO2 concentrations in the same order, which explains a non-linearity parameter α the same. The layer thickness of each peak becomes thin with SnO2 concentration to result the threshold voltage decrease and leak current increase with increasing SnO2 [2]. 1. 2.
H. Saijo and M. Shiojiri, in “Proc. 16th Intern’l Micros. Congr. Sapporo”, Vol. 2 (2006), p. 883. 2. N. Daneu, A. Recnik, S. Bernik and D. Kolar, J. Am. Ceram. Soc., 83 3165 (2000).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 361–362, DOI: 10.1007/978-3-540-85226-1_181, © Springer-Verlag Berlin Heidelberg 2008
362
Figure 1. Block Diagram of CL Microscope
Figure 2. CL observation of SnO2 0.1% and Bi2O3 1% doped ZnO varistor.
Figure 3. CL observation of SnO2 10% and Bi2O3 1% doped ZnO varistor. 1; SEM image, 2; CL micrograph of 1, 3-8; CL spectra of points marked in 1.
363
Study of structural properties of Mo/CuInS2/ZnS used in solar cells by TEM J. Sandino1, G. Gordillo2, H. Lichte1 1. Triebenberg Laboratory, Institute of Structure Physics, Technische Universitaet Dresden, D-01062 Dresden, Germany 2. Departamento de física, Universidad Nacional de Colombia, Bogotá, Colombia [email protected] Keywords: TEM, Thin films solar cells, structural properties, TEM
One of the steps to improve the efficiency of thin film solar cells is the exhaustive comprehension of the physical aspects present in the bulk of materials and their interphases. TEM is a tool that provides significant information about the specimen, by means of e.g. analysis of crystalline structure, defects visualization, grain boundaries and interfaces, and composition mapping. Additionally, Electron Holography allows measuring the inner potentials and electric fields [1], which will be decisive for the performance of thin films solar cells. Here, solar cells consisting of Mo/CuInS2/ZnS are investigated (Figure 1). CuInS2 has potential advantages in comparison with the most widely investigated selenium containing chalcopyrites. These include the significantly reduced toxicity of sulfur compared to selenium, which minimizes environmental impacts and facilitates mass production handling; furthermore, fabrication can be performed with short processing times and low thermal budget, quite appropriate for commercial application. The energy gap of the CuInS2 is close to the ideal one (1.5 eV) for a single junction solar cell [2]. For the performance of the solar cells, grain size distributions, composition of each layer, and structural mismatch between the different layers have a fundamental importance. For example, in the XRD spectra of a CuInS2-layer [4], obtained under variation of the incidence angle between 1.5 and 4º (see Fig. 2), only reflections corresponding to the In2S3 and CuInS2 phases appear. This indicates that a Cu2S phase is formed predominantly at the bottom of the sample, whereas In2S3 and CuInS2 phases grow in the whole volume [2]. For a more detailed analysis, a TEM investigation is needed. For this work, Mo/CuInS2/ZnS thin films were prepared with different deposition methods of the ZnS-layer, in order to analyze their influence on structural and electrical properties under TEM and Electron holography. The multilayer Mo/CuInS2/ZnS system in both samples was sequentially prepared on a substrate consisting of soda lime glass. First, Mo was deposited by DC magnetron sputtering with a S-gun configuration electrode. Next, for CuInS2, two sequential steps using elemental sulphur evaporated from an effusion cell, and metallic precursors of Cu and In evaporated from tungsten boats were used. Finally, ZnS was deposited by CBD (chemical bath deposition) and by co-evaporation, respectively. The CBD-deposited ZnS was grown from the following chemical bath composition [zinc acetate] = 15×10-3 M; [sodium citrate] = 7.5×10-3 to
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 363–364, DOI: 10.1007/978-3-540-85226-1_182, © Springer-Verlag Berlin Heidelberg 2008
364
60×10-3 M; [ammonia] = 300×10-3 M; [thiourea] = 150×10-3 M. Alternatively, a coevaporated ZnS-layer was grown from elemental evaporation sources; a detailed description of the process of deposition of each layer is given in [3]-[6]. Finally, the samples were prepared by traditional cross-sectioning and by FIB, and the TEM and HTEM measurements were accomplished using a CM200 ST/Lorentz Philips TEM. First results are shown in Figures 3-4. [7]. 1. 2. 3. 4. 5. 6. 7.
P.Simon, H. Lichte, D. Mönter, W. Reschetilowski, A. Valera, and W. Carrillo-Cabrera, 631, ZAAC (2005), p.983. N. Meyer, I. Luck, U. Ruehle, R. Klenk, M. C. Lux-Steiner, R. Scheer, Proc. 19th European Photovoltaic Solar Energy Conference, Munich, 2004, p.1698 G. Gordillo; F. Mesa; C. Calderón, Brazilian Journal of Physics 36 (2006), p. 982. J. Clavijo, E. Romero, J. S. Oyola and G. Gordillo, Proc. 22nd European Photovoltaic Solar Energy Conference, 2007, p. 2279. M. Ladar, E.J. Popovici, I. Boldea, R. Grecu, E. Indrea, Journal of Alloys and Compounds, 434 - 435 (2007) 697-700 G.Gordillo, E. Romero, Thin Solid Films 484 (2004) p.352 We kindly acknowledge supply of samples by the group of Materiales Semiconductors y Energía Solar de la Universidad Nacional de Colombia, financial support of the agreement ALECOL and DAAD. Discussions within the Triebenberg lab were indispensable.
InS CuS
ZnS CuInS2 Molybdenum Subtract (soda-lime glass)
Figure 1. Scheme of the Mo/CuInS2/ZnS system. Drawing is not to scale.
Figure 2. XRD spectra measured under small angle incidence for a CuInS2 film ZnS
CuInS2
Mo
Figure 3. TEM micrograph of the CuInS2 thin films analyzed.
0 1µm 1 0µm
1 1µm
Figure 4. TEM micrograph of the Mo/CuInS2/ZnS system prepared by CBD.
365
Texture analysis of silicide thin films: combining statistical and microscopical information H. Schletter1, S. Schulze1, M. Hietschold1, K. De Keyser2, C. Detavernier2, G. Beddies1, A. Bleloch3, and M. Falke1 1. Institute of Physics, Chemnitz University of Technology, 09107 Chemnitz, Germany 2. Department of Solid State Physics, Ghent University, 9000, Belgium 3. SuperSTEM Laboratory, Daresbury, WA4 4AD, Cheshire, UK [email protected] Keywords: EBSD, texture, SEM
The statistical distribution of grain orientations in a poly-crystalline thin film, called texture, is an important characteristic. The presence of preferred orientations is important for the macroscopical behaviour of the film due to an anisotropy of certain properties, like resistivity, carrier mobility, etc. Therefore it is important to know, which types of texture evolve for a certain combination of substrate and film material and in which way they depend on the sample preparation. In our measurements, electron backscatter diffraction (EBSD) was used to reveal the texture of the films. On one hand side, this technique provides good statistical data, because a large number of grains (in the order of 10³) is examined. On the other hand, because the measurement is carried out in an SEM, the information about grain orientation is available for every single point on the sample surface. Therefore, direct correlations between texture components (statistical data) and film morphology (microscopical data) can be drawn. As an additional source of information, high resolution TEM investigations were carried out. These measurements verify the EBSD results and reveal the interface structure at an atomic scale. The samples we investigated consisted of thin films (approximate thickness d = 50 nm) of CrSi2 and MnSi1 7 on Si(001) single crystal substrates. The films were grown by reactive codeposition on the heated substrate under UHV conditions. For some samples, a very thin metal layer was deposited as a template prior to the film growth. We found different kinds of texture present in all samples. Besides the various known epitaxial relations [1], we could identify new crystal orientations which belong to epitaxy, fiber texture and axiotaxy. The statistical data are visualized in pole figures. An example for CrSi2 is shown in Figure 1. The lines of high intensity, which are not concentric in the pole figures, are of special interest for us, since they refer to axiotaxial alignments. This orientation was identified as a new type of texture only a few years ago [2]. For CrSi2, the axiotaxial relation is CrSi2{100}||Si{110}. For MnSi1 7, two different axiotaxial orientations were found, namely MnSi1 7{118}||Si(110) and MnSi1 7{110}||Si(110). By analysing grain orientation maps (shown in Figure 2) and the corresponding SEM images, a correlation between texture components and grain size was found. The
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 365–366, DOI: 10.1007/978-3-540-85226-1_183, © Springer-Verlag Berlin Heidelberg 2008
366
pictures show, that the largest grains have an epitaxial orientation while randomly oriented grains have the smallest size on average. Therefore we conclude that the different texture components correspond to different growth conditions for the crystallites. 1. 2.
O. Filonenko et al., Journal of Crystal Growth 262 (2003), 281 C. Detavernier et al., Nature 426 (2003), 641
Figure 1. Statistical pole figure of CrSi2 (left) + theoretical lines for axiotaxy and spots for epitaxy (right).
Figure 2. Corresponding grain orientation map (different colours / grey levels represent different CrSi2 crystal planes being parallel to the silicon substrate surface).
367
Statistical Tomography of 3D Thin Film Structure using Transmission Electron Microscopy E. Spiecker1,2, V. Radmilovic2 and U. Dahmen2 1. Faculty of Engineering, Christian-Albrechts-University Kiel, Kaiserstrasse 2, 24143 Kiel, Germany 2. National Center for Electron Microscopy, Lawrence Berkeley National Laboratory, Berkeley, USA [email protected] Keywords: thin films, transmission electron microscopy, tomography
Thin films play a crucial role in many modern technologies, like microelectronics, solar cells, sensors, and coatings. A key to understanding and controlling thin film growth processes and properties is the knowledge of the variation in structure with distance from the substrate. Therefore experimental techniques for quantitative characterization of the three-dimensional (3D) structure of thin films are highly demanded. Transmission electron microscopy (TEM) is well established as a powerful tool for investigation of thin film structures down to the nanometer scale. However, cross-section and plan-view geometries commonly used in TEM studies of thin films are not suited for quantitative evaluation of 3D data since these geometries represent only two particular 2D sections through the film. On the other hand most film structures are much too complicated for application of standard 3D tomography techniques. We have recently developed a new sample preparation technique that overcomes these limitations by a double wedge geometry that probes different depths in the film and separates depth information in a continuous series of thin slices that are spread over a lateral distance [1,2]. The key steps of the preparation are (i) the formation of an ultrashallow dimple (slope ~ 0.1º) in the film surface, (ii) the determination of the dimple profile, and (iii) the formation of a small-angle wedge whose edge intersects the center of the dimple (Fig. 1). Along the edge of the double-wedge sample quasi-horizontal 2D sections at different film depths can be analyzed by plan-view TEM over large areas, thus enabling a statistical description of the 3D film structure. Fig. 2 depicts results of an application of this technique to a 3C-SiC film with columnar grain structure [2]. By evaluating more than 1800 grains in TEM images of a double-wedge sample the grain size distributions at six different height levels in the film have been determined with good statistics (Fig. 2b). From these data the evolution of the mean grain size could be determined (Fig. 2c) and, for the first time, the self-similarity of the grain size distribution, predicted earlier by computer simulations of faceted film growth [3,4], could be confirmed experimentally (Fig. 2d, for details see [2]). An alternative way of representing the results of the statistical analysis is shown by Fig. 2e which depicts an “average grain”. This kind of statistical tomography reconstructs average film morphologies from statistical analysis of large-area 2D sections in different film depths.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 367–368, DOI: 10.1007/978-3-540-85226-1_184, © Springer-Verlag Berlin Heidelberg 2008
368
1. 2. 3. 4. 5.
E. Spiecker, Phil. Mag. 86, 4941 (2006). E. Spiecker, V. Radmilovic, U. Dahmen, Acta Mater. 55, 3521 (2007) M. Grujicic and S.G. Lai, J. Mater. Synt. Proc. 8, 73 (2000). P. Smereka, X. Li, G. Russo, and D.J. Srolovitz, Acta Mater. 53, 1191 (2005). This work is supported by the AvH-Foundation and by the DOE (DE-AC02-05CH1123).
Figure 1. Schematic showing the geometry of a double-wedge sample for statistical 3D analysis of thin film structure. Along the sample edge the thin film structure can be investigated at each depth over large areas by plan-view TEM (see Ref. [2]).
Figure 2. Statistical analysis of the 3D grain structure of a polycrystalline SiC-film with columnar grain structure by large-area evaluation of TEM images of a double-wedge sample. Figure part e) depicts an “average grain” which has been reconstructed from the statistical grain size data (see Ref. [2]).
369
Analytical TEM investigations of Pt/YSZ interfaces V. Srot1, M. Watanabe2, C. Scheu3, P.A. van Aken1, E. Mutoro4, J. Janek4 and M. Rühle1 1. Max Planck Institute for Metals Research, Heisenbergstr. 3, Stuttgart, Germany 2. National Center for Electron Microscopy, Lawrence Berkeley National Laboratory, 1 Cyclotron Rd., Berkeley, CA94720, USA 3. Department Physical Metallurgy and Materials Testing, University of Leoben, FranzJosef-Straße 18, Leoben, Austria 4. Institute of Physical Chemistry, Justus-Liebig-University Gießen, Heinrich-Buff-Ring 58, Gießen, Germany [email protected] Keywords: metal-ceramic interfaces, EDXS, EELS
Metal-ceramic interfaces are of fundamental importance for a variety of industrial applications and are also of scientific interest. The physical and chemical properties of several technologically relevant nano-structural materials and devices are strongly affected and controlled by the presence of interfaces between the components. Already small amounts of impurities at the interface can dramatically change the properties of the system. Zirconia (ZrO2) is an industrially important ceramic material with a wide range of applications. Due to large volume changes during phase transitions, pure zirconia cannot be used as a high-temperature structural ceramic without stabilisation. Yttria (Y2O3)-stabilised zirconia (YSZ) is an extremely tolerant material with many interesting properties and applications [1]. In solid state electrochemistry platinum (Pt) is a highly important material for electrodes and as potential catalyst films [2]. The aim of our work was the investigation of Pt/YSZ interfaces using analytical transmission electron microscopy (TEM) techniques in order to detect any possible changes (diffusion, segregation…) across the interfaces. For our study Pt films were deposited on the (111) and (100) surfaces of YSZ single crystals using pulsed laser deposition (PLD). The dense and well oriented Pt layers were formed during the thermal treatment at 1023 K [3]. Scanning transmission electron microscopy (STEM) images revealed that the Pt films deposited on the (111) surface of YSZ have a thickness of about 100 to 150 nm and the Pt films on (100) YSZ surface are ca. 1 μm thick (Figure 1). The analytical TEM investigations of Pt/YSZ interfaces included energy-dispersive X-ray spectroscopy (EDXS) and electron energy-loss spectroscopy (EELS). In order to detect any possible variations across the Pt/YSZ interfaces we have performed several EDXS line-scan measurements in the samples with both substrate orientations. At every beam position intensities of the Zr-K, Y-K and Pt-L X-ray emission lines were measured. For the quantitative analysis of EDXS measurements, the new ζ-factor method introduced by Watanabe and Williams [4] was applied. According to our experimental results neither diffusion nor segregation could be detected across the S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 369–370, DOI: 10.1007/978-3-540-85226-1_185, © Springer-Verlag Berlin Heidelberg 2008
370
Pt/YSZ interfaces for both investigated YSZ orientations (Figure 2). Additionally the line-scan measurements across the domain boundaries in Pt films with the (111)Pt / (100)YSZ orientation showed that no detectable amounts of elements except Pt were present. The Pt/YSZ interfaces were additionally examined using EELS. Spectra were recorded in the energy ranges of O-K, Y-L2,3, Zr-L2,3 and Pt-M4,5 edges. In order to predict possible atomic models of the investigated interfaces ab initio full multiple scattering FEFF [5] calculations were performed and will be discussed. 1. 2. 3. 4. 5.
A. Navrotsky, Journal of Materials Chemistry 15 (2005), 1883-1890 B. Luerßen et al., Angew. Chem. Int. Ed. 45 (2006), 1473-1476 G. Beck et al., Solid State Ionics 178 (2007), 327-337 M. Watanabe & D.B. Williams, J. Microscopy 221 (2006), 89-109 A.L. Ankudinov et al., Physical Review B 58 (1998) 7565-7576
Figure 1. Bright field STEM images of Pt/YSZ interfaces of a) (111)Pt / (111)YSZ and b) (111)Pt / (100)YSZ investigated orientations.
Figure 2. EDXS line-scan measurement across the (111)Pt / (100)YSZ interface is shown. The values of Zr, Y and Pt atomic fractions are plotted versus the distance from the interface (IF).
371
Microstructure and self-organization of nano-engineered artificial pinning centers in YBa2Cu3O7-x coated conductors T. Thersleff1, E. Backen1, S. Engel1, C. Mickel1, L. Molina-Luna2, O. Eibl2, B. Rellinghaus1, L. Schultz1, B. Holzapfel1 1. IFW – Dresden, Institute for Metallic Materials, Postbox 270116, 01171 Dresden 2. University of Tübingen, Auf der Morgenstelle 10, D-72076 Tübingen, Germany [email protected] Keywords: TEM, FIB, artificial pinning centers, YBCO, 2411, PLD, Moiré
The introduction of nano-sized Artificial Pinning Centers (APCs) to YBa2Cu3O7-x (YBCO) coated conductors immobilizes flux lines at higher fields, thus increasing their usefulness and commercial applicability. Moreover, careful nano-engineering of these APCs facilitates the fine-tuning of the superconducting properties of coated conductors such as enhanced pinning along specific crystallographic orientations or an overall reduction in anisotropy [1]. Understanding the self-organizational behavior of these APCs and their effect on the superconducting properties of YBCO thin films is the focus of this work. TEM lamellae from samples prepared on single crystal SrTiO3 and LaAlO3 substrates using both Pulsed Laser Deposition (PLD) and Chemical Solution Deposition (CSD) methods incorporating APCs were produced using a Carl Zeiss 1540XB Focused Ion Beam (FIB) employing the in-situ lift-out method. TEM investigations on a FEI Tecnai T20 were carried out to elucidate the effect of the processing parameters on the organizational behavior of APCs and subsequently correlate this to the macroscopic properties of these films. The first pinning centers to be introduced are the so-called 2411 phase (Y2Ba4CuMOx where M = metal) into the YBCO matrix using the quasi-multilayer PLD approach described in [2]. Initial TEM investigations looked at the microstructure of YBCO / Y2Ba4CuZrOx (2411-Zr) quasi-multilayers deposited using an off-axis geometry described in [3]. The high resolution image shown in figure 1 indicates that a strong Moiré contrast is present with a spacing of about 2 nm, which may be indicative of a columnar defect structure caused by the presence of either 2411-Zr or BaZrO3 (BZO) nano-particles. Dark-field images were also taken in various orientations. Some results from the (100) reflection are shown in figure 2, which reveals a mixed rotational and lattice constant Moiré. A detailed chemical analysis of the sample was not completed at the time of abstract submission. 1. 2. 3.
S. R. Foltyn et al., Nature Materials 6 (2007) p. 631-642 J. Haenisch et al., Appl. Phys. Lett. 86 (2005), p. 122508/1-3 B. Holzapfel et al., Appl. Phys. Lett. 61 (1992) p. 3178
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 371–372, DOI: 10.1007/978-3-540-85226-1_186, © Springer-Verlag Berlin Heidelberg 2008
372
YBCO (001)
Moiré
YBCO (100)
2 nm-1
c-axis
Figure 1. High-resolution micrograph of YBCO / Zr-2411 quasi-multilayers in the [100] pole with a defocus close to zero Scherzer focus. The sample surface is located in the upper direction. The FFT subset reveals both the YBCO structure as well as the presence of Moiré reflexes, corresponding to a spacing of approximately 2.0 nm in real space.
Figure 2. Dark field image in the YBCO (100) reflection revealing the presence both mixed and lattice constant Moiré contrast.
373
The determination of the interface structure between ionocovalent compounds: the general case study of the Al2O3-ZrO2 large misfit system G. Trolliard, D. Mercurio SPCTS - UMR6638, 123 Av. Albert THOMAS, 87060 Limoges Cedex – France gilles.trolliard@unilim fr Keywords: thin films, interface structure, epitaxy
Electron microscopy is known to be a powerful tool to investigate the structure of crystalline interfaces. Many studies have been carried out with great success to analyze interfaces and defects at the atomic scale in metals or covalent semi-conducting materials. The atomic structure of oxide-oxide interfaces is however far much unknown. HREM observations of interfaces in aligned eutectics demonstrate that complex oxides, such as Al2O3 and ZrO2, can fit along particular crystallographic planes perpendicular to the interface [1]. More recently, we presented the results of a study devoted to the establishment of the interface crystallographic models of such oxides [2]. In this communication we propose an approach to determine the interface models in oxides, based on an HREM approach. The method is proposed in the case of large misfit systems which represents the general case study and should therefore be applicable to all kinds of complex oxide-oxide interfaces. With this aim, the ZrO2-Al2O3 system has been chosen as no intermediate phase could be formed within the interface. In addition, the solid solution occurring between these two compounds is usually very limited in composites produced by conventional methods. Thus the zirconia-alumina system can be considered as non-reactive interface. The studied samples are synthesized by the sol-gel route, which allows growing thin monoclinic zirconia islands of pure zirconia showing a heteroepitaxial growth on (112 0)sa rhombohedral single crystal sapphire substrates. Their heteroepitaxial relationship is first established by electron diffraction on plane view samples (Fig. 1). Different orientation variants were determined. Specific transverse sections where then elaborated by careful selection of the substrate orientation on the base of XRD experiments. They were then prepared normal to the in-plane common directions of the two crystals. In a second step, the metric of the coincidence super-cell between the two lattices was obtained by these HREM images. Indeed, whatever the orientation variant, the HREM images of the interfaces reveal the occurrence of super-periodicities corresponding to common planes across the interface, that account for a full structural continuity between the two phases (Fig. 2). Finally, the geometry of the interfacial coordination polyhedra is deduced and presented as a 3D interface model (Fig. 3). This communication will present the results obtained both on the main orientation variant, corresponding to the most commonly observed variant, and on a secondary orientation variant which is more seldom seen.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 373–374, DOI: 10.1007/978-3-540-85226-1_187, © Springer-Verlag Berlin Heidelberg 2008
374
Figure 1. Monoclinic zirconia island showing heteroepitaxial relationship with the alumina substrate. 3d (-101) ZrO2
ZrO2
Al2O3
8d(11 08)Al2O3
Figure 2. Bragg filtered image obtained on the secondary variant and showing the supercell periodicity.
Figure 3. Interface model of the main orientation variant. Specific polyhedra in which the zirconium cation is 7-fold coordinated are involved to build up the interface between alumina and zirconia.
It is shown that the orientation relationship is governed by the occurrence of the common planes crossing the interface, observed in the HREM images (Figs. 2, 3). These common planes are clearly attributed to common cationic planes of both ZrO2 and Al2O3. They correspond to ‘structural walls’ within which the cationic lattices of the two phases are similar and thus perfectly coherent, explaining the continuity across the interface. Alumina-zirconia represents a case of large misfit system. However, except the expected geometrical dislocations and ledges (Fig. 2), the interfaces present very few physical defects. The overall interfacial polyhedra of coordination however suffer high distortions. The lattice mismatch could thus be locally accommodated by an important elastic strain linked to fluctuations of the cation-anion interatomic distances. The predominance of this relaxation mechanism based on the adaptability of the ionocovalent bonds seems a characteristic of oxide-oxide interfaces. 1. 2.
L. Mazerolles, D. Michel, M. Hÿtch, J. Eur. Ceram. Soc.; 25, (2005), 1389-1395 G. Trolliard, R. Benmechta, D. Mercurio and O.I. Lebedev; J. Mater. Chem., 16, 36, (2006), 3640 – 3650
375
Simple method to improve quantification accuracy of energy-dispersive X-ray spectroscopy in an analytical transmission electron microscope by specimen tilting T. Walther Department of Electronic & Electrical Engineering, University of Sheffield, Sir Frederick Mappin Building, Mappin Street, Sheffield S1 3JD, UK [email protected] Keywords: microanalysis, X-ray, energy-dispersive X-ray spectroscopy (EDXS), specimen tilt
The accuracy of measurements of elemental concentrations by energy-dispersive Xray spectroscopy (EDXS) depends on the knowledge of the ionisation cross-sections of the corresponding elements (Z-effect) [1, 2] and proper corrections for absorption (A) [3] and for fluorescence (F) [4]. These effects are now routinely combined for given specimen thickness and density in the so-called ZAF-correction. More recently, fully self-consistent spectrum modelling has become available which models X-ray generation as a function of mass-thickness and then integrates the result over the specimen thickness, e.g. with the PROZA96 software package [5]. If a structure to be analysed is much smaller than the sample thickness, however, two further factors become relevant, namely electron beam broadening [6, 7] and the top-bottom effect, i.e. the depth position of the feature within the foil, as X-rays going through a thicker part of the sample before reaching the detector will be absorbed more strongly. The further a feature is located within the foil towards the bottom surface, the fainter the X-ray signal recorded from it. If this depth position could be measured experimentally it could be taken account of in the absorption correction. Here I show this can be determined indirectly, taking two measurements for different specimen tilts. For a thin layer embedded at depth d within the foil, Figure 1 shows that X-rays from the thin layer have to travel a distance D=d/sin θ through the sample to reach the detector. Hence, for two take-off angles θ1 and θ2 the X-ray path length difference is (1). D2–D1 = d (1/sinθ2–1/sinθ1) The X-ray intensity I for any given element will decay exponentially with the effective path length D, with some attenuation wavelength λ, i.e. for measurements at two different take-off angles θ1 and θ2 and thus different path lengths D1,2: (2) I1,2 = A exp(–D1,2/λ) The intensity ratio then is given by I1/I2 = exp[(D2–D1)/λ] (3) which can be solved for D2–D1 = λ ln(I1/I2) (4). A comparison of equations (1) and (4) with some trigonometry finally yields [8]: d = 4λ ln(I1/I2) sin[(θ1–θ2)/2] cos[(θ1+θ2)/2] /{[cos[(θ1–θ2)] – cos[(θ1+θ2)]} (5) This means one can calculate the depth of the feature in a foil from the intensity ratio of
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 375–376, DOI: 10.1007/978-3-540-85226-1_188, © Springer-Verlag Berlin Heidelberg 2008
376
two X-ray measurements using the attenuation wavelength λ, the angular difference (θ1–θ2) that can directly be read from the goniometer stage and the average value (θ1+θ2)/2 that can be obtained from the manufacturer of the X-ray detector. With the knowledge of d, the absorption/fluorescence correction for the top-bottom effect can then be refined if either experimental or calculated values of λ are available. As an example, Monte Carlo simulations of electron scattering and X-ray generation as a function of foil thickness have been carried out using the CASINO software (version 2.4.2) [9, 10] to model the absorption effect to a first (non-relativistic) approximation and determine some tentative values of typical attenuation lengths. Figure 2 depicts plots of the calculated X-ray intensities of lines for the case of 2nm thin layers at different depths d within 200nm of GaAs. Elements that can occupy substitutional lattice sites in the III/V semiconductor GaAs and are technologically relevant (i.e. N, Al, P, In and Sb) have been included. Linear regression analysis to logarithmic plots of I(d) yielded the following attenuation lengths: λ(NK)=122nm; λ(AlK)=319nm; λ(PK)=618nm; λ(InL)=2323nm; λ(SbL)=3009nm; λ(InK)=λ(SbK)=∞ for hard X-rays.
intensity [counts]
12 11
2nm thin film in 200 nm GaAs (x10)
10 9 8
Al_K P_K Sb_K
7 6 5
Sb_L In_K In_L N_K
4 3 2 1 0 0
Figure 1. Basic sketch of geometry, angles and distances used in the equations and their analytical solution
50
100 depth d [nm]
150
200
Figure 2. Plot of signal attenuation for 2nm thin layers of of N, Al, P, In or Sb if there is GaAs of thickness d between them and the Xray detector. U=200kV, take-off angle θ=90°
1. H.A. Bethe, Ann. Phys. 397 (1930) 325 2. P. Duncumb and S.J.B. Reed, in “Quantitative Electron Probe Microanalysis”, ed. K.F.J. Heinrich (NBS Spec. Publ., Washington) 298 (1968) 133 3. J. Philibert, Proc. Int. Symp. X-ray Optics and X-ray Microanalysis, ed. H.H. Pattee, V.E. Cosslett and E. Engström (Academic Press, New York) (1963) 379 4. S.J.B. Reed, Brit. J. Appl. Phys. 16 (1965) 13 5. G.F. Bastin, J.M. Dijkstra and H.J.M. Heijligers, X-ray Spectrom. 27 (1998) 3 6. J.I. Goldstein, J.L. Costley, G.W. Lorimer and S.J.B. Reed, Proc. Workshop Anal. Electron Microsc., ed. O. Johari (IIT Research Institute, Chicago) 1 (1977) 315 7. P.A. Crozier, M. Catalano and R. Cingolani, Ultramicroscopy 94 (2003) 1 8. T. Walther, Proc. EMAG conference, Glasgow (2007) in print 9. P. Hovington, D. Drouin and R. Gauvin, Scanning 19 (1997) 1 10. P. Hovington, D. Drouin, R. Gauvin, D.C. Joy and N. Evans, Scanning 19 (1997) 29
377
Comparison of transmission electron microscopy methods to measure layer thicknesses to sub-monolayer precision T. Walther Department of Electronic & Electrical Engineering, University of Sheffield, Sir Frederick Mappin Building, Mappin Street, Sheffield S1 3JD, UK [email protected] Keywords: Energy-dispersive X-ray spectroscopy (EDXS), wetting layer, grain boundary width
Energy-dispersive X-ray spectroscopy (EDX) is an analytical tool to measure the chemistry of thin layers in cross-sectional transmission electron microscopy (TEM). Two methods are compared here using Monte Carlo simulations of electron scattering and X-ray generation as a function of foil thickness by the CASINO software [1]: 1. scanning TEM (STEM) line profiles recorded by scanning a focused electron beam across the layer oriented edge-on: the effective density of atoms within the layer is given by the integral of the measured profile which can be directly calculated up to a certain extent (method 1a) or modelled using Gaussian distributions (method 1b). 2. series of nano-probe TEM illuminations with different beam diameters. The effective layer thickness can be determined from a least-squares fit of atomic ratios plotted as a function of beam diameter; in the following this is called method 2 [2]. The model consists of ½ unit cell of InAs (i.e. 1 monolayer (ML) of In atoms or d=0.14nm) sandwiched between GaAs, imaged edge-on using 200kV electrons and an X-ray detector at 20° take-off angle. For fair comparison the number of electrons in the simulations have been the same for both methods (dose: 1.2×107 e–), distributed either over 100 STEM probes (diameters 2r=0.14, 0.5 or 2nm) or a dozen TEM illumination spots of radii r = 7, 10, 13,…, 40nm. Specimen thicknesses considered were t = 48, 100 and 197nm. From thin bulk InGaAs k-factors for the relative intensities of the X-ray lines have been determined as kInK/GaK=0.351 and kInL/GaL=1.284. These were used, after elimination of some program bugs [3], to convert intensity ratios into atomic % [4]. The apparent widths (FWHM) of the scanned profiles were 0.4nm, 1.5nm and 5nm. Table 1 demonstrates that methods 1a and 1b yield inconsistent results and that their output values scatter by a factor of ~2, without any possibility to guess how reliable a particular measurement would be. Table 2 shows that in method 2, large thicknesses introduce non-linearities due to the effect of beam broadening, which degrades the fit quality. For small and intermediate thicknesses the linear fit is excellent, however. Here, if R2>0.9 then the output of both K- and L-lines is highly accurate. In this case the average d=136±19pm, where the error bar contains statistical and systematic errors [3], corresponds to 0.97±0.14 ML and is a reliable measure of the input value of 1 ML. 1.
P. Hovington, D. Drouin and R. Gauvin, Scanning 19 (1997) 1
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 377–378, DOI: 10.1007/978-3-540-85226-1_189, © Springer-Verlag Berlin Heidelberg 2008
378 2. 3. 4.
T. Walther, J. Microsc. 215 (2004) 191 and 223 (2006) 165 T. Walther, Proc. EMAG2007, Glasgow (2007) in print S.J.B. Reed, Ultramicroscopy 7 (1982) 405 10000
InL @ t=48nm
intensity [counts]
InL @ t=100nm
1000
InL @ t=197nm
Figure 1. Profiles of In and Ga L-line intensities vs. STEM probe position for 0.14nm wide electron beam and different thicknesses. Please note the logarithmic intensity scale.
GaL @ t=48nm 100
GaL @ t=100nm GaL @ t=197nm
10
-2.2
-1.2
1 -0.2
0.8
1.8
probe position [nm]
Table 1. Effective chemical layer width d [pm] determined from STEM profiling for three probe sizes (diameter 2r) and sample thicknesses (t) using k-factors for K- and Llines as described. Input chemical width: dtrue=140 pm. Labels (a) and (b) refer to methods 1a and 1b, respectively. Mean values for each row are given in the last column. t [nm] 48 100 197
2r [nm] X-ray lines K L K L K L
0.14 (a) (b) 199.8, 181±30 187.2, 175±29 170.4, 149±25 159.1, 142±24 139.2, 119±20 131.0, 113±19
0.5 (a) (b) 193.9, 119±40 175.2, 108±36 173.0, 167±33 154.7, 152±30 140.7, 160±27 128.3, 123±25
GaK / InK ratio * 0.351
t = 48 nm 100 nm 197 nm
400
200
0 0
5
10
15
∅ 173±30 173±34 166±16 148±24 138±29 124±26
Table 2. Effective chemical layer widths d [pm] from method 2 for various sample thicknesses t and ratios of Ga/In K- or L-line intensities after k-factor correction. R2 is linear correlation coefficient.
800
600
2 (a) (b) 182.2; 160±40 204.6; 189±38 189.4, 145±29 176.3, 104±26 176.1, 95±24 163.2, 84±21
20
25
30
35
40
beam radius r [nm]
Figure 2. Plot of the k-factor corrected Ga/In ratio of the K-lines as a function of beam radius. The results for L-lines are very similar.
t R2 0.88 0.91 0.96 [nm] X-ray lines 48 K 143±14 L 127±12 100 K 147±21 L 129±19 197 K 102±18 L 93±16
379
Determination of interface structure of YBCO/LCMO by a spherical aberration- corrected HRTEM Z.L. Zhang1, U. Kaiser1, S. Soltan2 and H.-U. Habermeier2 1. Materials Science Electron Microscopy, University of Ulm, 89069 Ulm, Germany 2. Max-Planck-Institut für Metallforschung, D-70569, Stuttgart, Germany [email protected] Keywords: Cs-corrector, HRTEM, interface
Heterostructure interface plays an important role in modern microelectronics, which could be effectively used to control various electronic and magnetic properties by tuning the atomic structure and chemical composition of the interfaces. The interface also creates new and unexpected phenomena produced by the strong interaction among the electrons. Heterostructure interfaces consisting of superconducting and ferromagnetic manganese oxide attract much attention recently [1-3]. Generally, a chemically pure and atomically sharp interface is needed for achieving particular properties. However, to visualize the atomic structure of interface consisting of light and strong scatters with high precision in detail is only possible by applying spherical-aberration correction techniques [4-5]. Figure 1 is an representative HRTEM image of one interface of a bi-layer heterostructure YBCO(YBa2Cu3O7-δ)-LCMO(La2/3Ca1/3MnO3)-YBCO, which was acquired by an objective-lens Cs-corrected Titan FEI 80-300 microscope under a CS of -1.0 µm and small over-focus. The image indicates a perfect epitaxial relationship along the caxis due to extreme low mismatch. The orientation relationships in between are: YBCO [001] //LCMO [001] and YBCO [100]//LCMO [110]. Under this condition atoms in the adjacent two layers and the interface are clearly visible and imaged as white atoms, which enable to readily determine the atom types combined with atomic model. Further analysis reveals that the interface is composed of CuO plane and –LaCaO plane. Oxygen atom column contrast is clearer and stronger in the LCMO layer than in YBCO layer. Oxygen contrast is not pronounced in CuO2 chain (but, detectable by line-profile) whereas it is remarkable in BaO chains. Using multislice method [6], simulated HRTEM images based on the atomic model are inserted, which demonstrates reasonable fitting with experimental contrast under similar experimental condition, therefore, corroborating the experimental contrast observed and atom configurations at the interface. Figure 2 shows the variations of plane spacing over a rectangular area about 3.0 nm by 1.5nm from position A to B. Closely examination on the spacing reveals that the interface spacing (denoted by arrow 1 and 2 ) is larger, 0.227nm, than the averaged value (denoted by arrow 5 and 6), 0.192 nm, in LCMO layer. Atom planes at the interface slightly expand compared to the adjacent atom planes. Further HRTEM study, combined with exit wave reconstruction, the whole three layer recorded in one image, reveals that such heterostructure usually exhibits two dis-
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 379–380, DOI: 10.1007/978-3-540-85226-1_190, © Springer-Verlag Berlin Heidelberg 2008
380
tinct interfaces, which are either CuO-LaCaO (as shown in Fig.1.) or BaO-MnO termination layers, one on each side of the LCMO layer. 1 2 3 4 5 6
J. Chakhalian, et al, Science 318(2007)1114. M. Varela, A.R. Lupini, S.J. Pennycook, et al, Solid-State Electronic. 47 (2003) 2245. T. Holden, H.-U. Habermeier, et al , Phy.Rev.B 69(2004)064505. M. A. O’Keefe, Ultramicroscopy 108 (2008) 196. L. Houben, A. Thust, K. Urban, Ultramicroscopy 106 (2006) 200. A. Chuvilin and U.Kaiser, Ultramicroscopy 104 (2005) 73.
Figure 1 (a) High-resolution image of the interface of YBCO/LCMO recorded under a negative CS (-1.0 µm) and defocus, where the LCMO terminates in a LaCa-O plane while YBCO terminates in CuO plane. The simulated image based on the atomic model (left) is inserted. Note that oxygen atom column contrast in CuO plane is weak.
Figure 2. Intensity traces across the interface over a rectangular areas (in Fig.1) illustrating the variation of plane spacing. It is clearly seen that a large spacing exist in the interface, i.e. 0.237 nm. The first neighbor atom planes both in YBCO and LCMO are somehow compressed, which reflect a smaller spacing relative to the averaged values.
381
HREM characterization of BST-MgO interface O.M. Zhigalina1, A.N. Kuskova1, A.L. Chuvilin2, V.M. Mukhortov3, Yu.I. Golovko3 and U. Kaiser2 1. Institute of Crystallography, Russian Academy of Sciences, 119333, Moscow, Russia 2. University of Ulm, Albert-Einstein-Alee 11, 89069, Ulm, Germany 3. South Scientific Centre, Russian Academy of Sciences, 344006, Rostov-on-Don, Russia [email protected] ras ru Keywords: films, ferroelectric, interface
It is known the properties of thin ferroelectric films can be different from bulk materials, that is concerned with an influence of mechanical stress (up to several GPa) at the film – substrate interface [1]. The stress can be partially (or fully) relaxed by means of misfit dislocation formation. So it is necessary to investigate both thin films and heterostucture interfaces at the atomic level to understand relationships between the microstructure and the electrical properties. High resolution electron microscopy (HREM) is a powerful method for the study of the film – substrate interface at the nanometer scale. Combined with geometric phase analysis, useful information can be obtained concerning local strains, variations in lattice parameters in the region of the film – substrate interface. Image analysis was carried out using especially written scripts for Digital Micrograph 3.5 (Gatan) [2]. For TEM and HREM investigations cross sections were prepared by both ion milling in Gatan PIPs 691 and focussed ion beam (FIB) technique in Quanta 200 3D (SMA Company). All samples were characterized in a Tecnai G2 30ST and a FEI Titan 80-300 at accelerating voltage of 300kV, using imaging, electron diffraction and highangle-annular dark-field (HAADF) STEM detector. (Ba0 8Sr0 2)TiO3 (BST) thin epitaxial films were deposited on [001]-oriented MgO substrate by rf sputtering. Recently it has been shown [3] the degree of stress in the epitaxialy grown thin films is a function of the film thickness. The method of geometric phase analysis was used to visualize local strains and extrinsic dislocations in the BSTMgO interface for films with different thickness (5 – 1000 nm). BST thin films revealed a monocrystalline structure with low-angle blocks boundaries (θ < 20) (Figure 1). The main reason of the block structure was a surface geometry (holes and hills) of MgO substrate. Digital analysis of cross sections HREM images (Figure 2) allowed us to visualize and compare misfit dislocations and displacement fields around their cores at the heterostructure interface for films with different thickness. It has been shown by Z-contrast STEM images and image simulation there are two possible ways of film-substrate atomic bonds at the BST-MgO interface: titan-oxygen or barium-oxygen. Analysis of dark field high resolution STEM images has indicated both variants of bonds can be observed.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 381–382, DOI: 10.1007/978-3-540-85226-1_191, © Springer-Verlag Berlin Heidelberg 2008
382
1. 2. 3. 4.
Y.S. Kim, D.H. Kim, J.D. Kim, et. al., Appl. Phys. Lett., 86 (2005), p.102907 A.K. Gutakovskii, A.L. Chuvilin, Se Ahn Song, Izvestiya RAS, ser. phys., 71 (2007) p.1464 P.-E. Janolin, Bo-Kuai Lai, Y.I. Yuzuk et. al., Book of abstracts EMF-2007 Bled, Slovenia p.74 The work was supported by RFBR grant № 07-02-12259-ofi and the State Program for Support of Leading Scientific schools, project № NSh-1955.2008.2. We kindly acknowledge SMA Company for the help in sample preparation.
Figure 1. High-resolution dark field image of the block boundary (white arrows) in BST thin film. Cross-section.
b) a)
c)
Figure 2. a) HREM image of BST-MgO interface; b) corresponding FFT; c) maps of variations of lattice parameters combined with (020) – filtered image displaying the (020) planes ending the interfacial dislocations.
383
TEM investigations on novel shape memory systems with Ni-depletions D. Schryvers, R. Delville, B. Bartova* and H. Tian EMAT, University of Antwerp, Groenenborgerlaan 171, B-2020 Antwerp, Belgium * now at Swiss Federal Institute of Technology (EPFL), CH-1015 Lausanne, Switzerland [email protected] Keywords: martensite, microstructure, precipitation
Many of today’s shape memory systems contain a substantial amount of Ni. The most typical system is of course Nitinol® based on the binary Ni-Ti alloy used near to its equiatomic composition. Another well known system is Ni-Al, which has been very thoroughly studied more for its fundamental physical characteristics rather than its practical applications. Recently, however, new ternary systems have attracted a lot of attention attempting to, e.g., introduce magnetic transitions and driving forces, such as in Ni-Mn-Ga or Co-Ni-Al or lower the hysteresis and increase the transformation temperatures in Ni-Ti-(Au,Pd,Pt), replacing mainly Ni with the ternary compound. At the same time, new studies have revealed unwanted Ni release in commercial wires for medical use. Focusing on Ni thus remains important for understanding the behaviour of martensitic transformations and shape memory applications. In the present lecture we will present results on the ternary system Ni50-xTi50Pdx in which different amounts of Pd substitution on Ni positions lead to special ratios between the austenite and martensite lattice parameters. As a result, the hysteresis of the transformation becomes very narrow and the amount of microtwinning, necessary to yield an invariant plane strain, decreases drastically. Also, when changing the amount of Pd, the type of stable microtwinning changes from Type I & II into compound. A first result is shown in Figure 1 demonstrating the change of microstructure as the content of Pd is decreased from 23 at.% (1.a) to 20 at.% (1.b) and 11 at.% (1.c) where the compatibility condition between austenite and martensite is satisfied. Detwinning and rearrangement of the martensite plates lead to a radically different microstructure which can account for the decrease of hysteresis [1]. Another system is the magnetic Co38Ni33Al29 with a Curie temperature above 90°C due to the replacement of mainly Ni by Co. Depending on the thermal treatment, nanoscale precipitates of fcc or hcp Co grow in the B2 matrix [2], as shown in Figure 2. Due to the large amount of these precipitates, they can seriously change the composition of the matrix thus affecting martensitic and magnetic transformation temperatures. In medical devices an oxide film is formed on the surface inhibiting leakage of toxic Ni into the human body. Even without special thermal treatments, a natural Ti-oxide films forms, which normally should not contain Ni. Recent work, however, has shown that in some cases pure metallic Ni particles can exist inside this Ti-oxide surface film, as seen in Figure 3. Also a Ni3Ti intermediate layer was observed. The composition and structure of the film is investigated by HRTEM, EELS and EFTEM techniques, with samples being prepared by FIB.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 383–384, DOI: 10.1007/978-3-540-85226-1_192, © Springer-Verlag Berlin Heidelberg 2008
384
1. 2. 3.
J. Cui, Y.S. Chu, O.O. Famodu et al., Nature Materials 5 (2006) 286-290 B. Bartova, D. Schryvers, Z. Yang, S. Ignacova and P. Sittner, Scripta Materialia 57 (2007) 37-40 We kindly acknowledge support of the projects FWO G.0465.05, FWO G.0180.08N, MULTIMAT MRTN-CT-2004-505226
Figure 1. Example of the changing microstructures observed in Ni50-xTi50Pdx samples.
Figure 2. (a) fcc Co precipitates observed in as-cast Co38Ni33Al29 material (1530°C, 10ms-1) and (b) hcp Co precipitates observed after a 4 hour annealing at 1275°C.
Figure 3. EFTEM revealing (a) metallic Ni particles (black) in the Ti-oxide film (whitegrey) of a cold-rolled Ni-Ti microwire and (b) an intermediate Ni3Ti layer between the metallic core and oxide surface.
385
Crystalline-to-amorphous transformation in intermetallic compounds by severe plastic deformation K. Tsuchiya1, T. Waitz2, T. Hara1, H.P. Karnthaler2, Y. Todaka3, M. Umemoto3 1. National Institute for Materials Science, Sengen 1-2-1, Tsukuba, Ibaraki 305-0047, Japan 2. Physics of Nanostructured Materials, University of Vienna, Boltzmanngasse 5, 1090 Vienna, Austria 3. Dept. of Production Systems Engineering, Toyohashi University of Technology, Tempaku-cho Hibarigaoka 1-1, Toyohashi, Aichi 440-8580, Japan tsuchiya [email protected] Keywords: shear band, twin, martensite
Process of nanostructure formation and crystalline-to-amorphous transformation (CTAT) by high pressure torsion have been studied for various intermetallic compounds, such as, TiNi, ZrCu and Ni3Al. These compounds have been chosen to elucidate the effect of crystal structure on CTAT. Crystal structures of the samples were B2 or B19’ martensite for TiNi, Cm martensite for ZrCu and L12 for Ni3Al. Discs (10 mmφ x 0.85 mm) were cut from a hot-rolled sheet (TiNi) or a casted ingot (TiNi, ZrCu and Ni3Al). After an adequate heat treatment for homogenization, the discs were deformed by high pressure torsion (HPT) apparatus up to 50 turns under an applied pressure of 5 GPa. For TEM observations, 3mmφ discs were cut from the deformed samples and electropolished by Tenupol. HRTEM observations were carried out using a CM 30ST operating at 300 kV. Nanobeam diffraction (NBD) study was done on a JEM-2010F operated at 200 kV. Complimentary X-ray diffractometry (XRD) and optical microscopy (OM) were also carried out. TiNi has been known to undergo CTAT by various SPD processes, e.g., cold rolling[1, 2], shot peening [3] and HPT[4]. We have pointed out that a drastic increase in lattice defects in shear bands is one of the dominant mechanisms of CTAT by cold rolling [2]. Fig.1(a) is a TEM bright field image of B2/amorphous lamellar often seen in HPT sample as well as in cold rolled samples. HRTEM observations and FFT analysis (Fig. 1(b)) indicate that the B2 crystals at the both sides of the amorphous band are in the same orientation. Such structures suggest that the martensitic twin boundaries are preferred site for defect accumulation and the CTAT starts at these boundaries. Long range order was retained even just before the CTAT. Fig.2(a) is an OM image of ZrCu after HPT deformation of 50 turns. Numerous shear bands can be seen running nearly parallel to the shear direction (denoted as SD) with many branching. Fig.2(b) shows a corresponding TEM image. The shear bands, which have very similar morphology to those observed in OM, are seen running nearly parallel to each other, but some of them also exhibit complex branching. Thicker bands exhibit some diffraction contrast but thinner ones seem to be rather featureless. It should be also noted that, compared to the case to TiNi the grains remain to be coarse and the dislocation density is not so high in the surrounding area of the deformation S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 385–386, DOI: 10.1007/978-3-540-85226-1_193, © Springer-Verlag Berlin Heidelberg 2008
386
bands. Fig.2(c) exhibits HREM of the deformation bands of a few nm width (denoted by the arrows). Detailed HREM observations and NBD study revealed that these nanoscale deformation bands are amorphous. On the contrary CTAT was not observed for Ni3Al even after HPT deformation of 30 turns; the sample remained to be nanocrystalline of about 50 nm. XRD results indicated significant decrease in the intensity of superlattice reflection was observed in the first few turns of HPT deformation as reported previously [5]. The process and mechanism of CTAT will be compared and discussed for these intermetallic compounds. 1. 2. 3. 4. 5.
J. Koike, D. M. Parkin, Journal of Meterials Research 5 (1990) 1414-1418. H. Nakayama, K. Tsuchiya, Z.-G. Liu, M. Umemoto, K. Morii, K. Shimizu, Materials Transactions 42 (2001) 1987-1993. D. M. Grant, S. M. Green, J. V. Wood, Acta Metallurgica et Materialia 43 (1995) 10451051. Y. V. Tat'yanin, V. G. Kurduymov, V. B. Fedorov, Physics of Metals and Metallography 62 (1986) 133-137. C. Rentenberger, H. P. Karnthaler, Acta Materialia 53 (2005) 3031-3040.
Figure 1. lamellar structures of Ti-50.2Ni HPT deformed for 2 turns. (a) TEM bright field micrograph and selected area electron diffraction (inset). (b) HREM image and corresponding FFT (inset).
Figure 2. microstructures of ZrCu HPT deformed for 50 turns. (a) optical micrograph. (b) TEM bright field image. (c) HREM image.
387
EELS quantification of complex nitrides in a 12 % Cr steel M. Albu1, F. Méndez Martin2 and G. Kothleitner1 1. Institute for Electron Microscopy, Graz University of Technology, 8010 Graz, Austria 2. Institute for Materials Science, Welding and Forming, Graz University of Technology, 8010 Graz, Austria [email protected] Keywords: nitride precipitates, EELS, quantification
In 9–12 % Cr steels, nitrides (MX, M2X and modified Z-phase ((Cr,V,Nb,Fe)N)) are of special interest because of their different contribution to the creep strength of the material. The changes in the chemical composition and their crystallography were investigated using transmission electron microscopy (TEM). The different phases have been identified by using the energy filtered TEM (EFTEM) technique [1] and the corresponding bivariate scatter diagrams of chromium and vanadium jump ratios (Fig. 1a-b). Their elemental composition has been established both with electron energy loss spectroscopy (EELS) and energy dispersive X-ray spectroscopy (EDX). Nevertheless the light elements are not easily quantifiable with EDX, for which reason EELS was involved. Furthermore, the energy-loss near edge structure (ELNES) of the nitrogen ionisation K edge has been used to differentiate between different metastabile nitride phases [2]. Analysis was carried out on a total of 60 thin particles from three differently treated samples: as-received (after tempering at 780 °C), thermally aged and creep loaded at 600 °C for 24 639 h at 115 MPa. The specimens were prepared by extracting the precipitates from the matrix into an amorphous carbon film. In the EEL spectra, edges coming from Nb(M45,M23), N(K), V(L23), Cr(L23) and Fe(L23) were recognised in addition to amorphous carbon from the extraction film. Since the edges from Nb, N, V and Cr are energetically too closely spaced and a conventional edge intensity extraction is not possible, the multiple linear least squares (MLS) fit deconvolution has been employed, fitting suitable references to all overlapping edges. Such an MLS fit together with the references used is shown in Fig. 2 for a mod. Z-phase particle. Computing the relative fit weights and integrating the references over an energy range of 100 eV, allows calculation of the atomic percentages of each element quite accurately, provided experimentally determined cross-sections [3,4] are available, as in this case. The mean elemental concentrations of precipitates under study i.e. the M2X, MX and modified Z-phase shows a good agreement comparing with the outcomes of the thermodynamic model implemented in the software package MatCalc (Table I) [5]. 1. 2.
I. Letofsky-Papst, P. Warbichler, F. Hofer, E. Letofsky, H. Cerjak: Z. Metallk. 95 (2004) 18. F. Hofer, P. Warbichler, A. Scott, R. Brydson, I. Galesic, B. Kolbesen: Journal of Microsc. 204 (2001) 166.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 387–388, DOI: 10.1007/978-3-540-85226-1_194, © Springer-Verlag Berlin Heidelberg 2008
388
3. 4. 5.
M. Albu, F. Méndez Martin, B. Sonderegger, G. Kothleitner: Int. Journal Mat. Res., in print F. Hofer: Microsc. Microanal. Microstruct. 2 (1991) 215. J. Svoboda, F.D. Fischer, P. Fratzl, E. Kozeschnik: Mater. Sci. Eng. A 385 (2004) 157.
200 nm
Figure 1. Phase diagram of a representative position from a creep loaded sample and the respective diffraction pattern from the mod. Z-phase –green particle. M23C6 –blue and MX(VN) –yellow were identified as well.
arb. units
V L23
Cr L23
NK
Nb M45
Nb M23
eV
Figure 2. MLS fit using Nb, N, V and Cr -references for a mod. Z-phase particle. With black colour is represented the experimental spectrum and with grey the MLS fit. Table I. Mean concentrations and their standard deviations from EELS measurements of M2X, MX and mod. Z-phase particles compared with the MatCalc simulations. EELS Cr (at.%) M2X 49.8 ± 3.4 MX 11.6 ± 4 mod. Z-phase 31.4 ± 4.2 Simulations M2X MX mod. Z-phase
Cr (at.%) 50.69 0.05 31.31
V (at.%) 17.2 ± 2.1 40.0 ± 4.5 30.1 ± 2.4
Nb (at.%) 6.9 ± 2.7 3.1 ± 1.6
Fe (at.%) 2.6 ± 1.7 1.7 ± 1.1 3.5 ± 1.2
N (at.%) 30.4 ± 4.2 41.2 ± 4.8 32.3 ± 3.4
V (at.%) 14.75 47.39 31.20
Nb (at.%) 1.04 5.40 3.45
Fe (at.%) 0.09 0.02 3.30
N (at.%) 32.87 46.61 30.70
389
Formation of ordered solid solution during phase separation in Cu-Ag alloy films F. Misják, P.B. Barna, G. Radnóczi Research Institute for Technical Physics and Materials Science (MFA) of the Hungarian Academy of Sciences, H-1525 Budapest, P.O.Box 49, Hungary [email protected] hu Keywords: coating, Ag-Cu alloy, phase separation, ordered solid solution
The Cu-Ag binary system belongs to the two component systems of practically non mixing components at thermodynamic equilibrium. At non equilibrium conditions however, substantial mixing could be observed. Cu–Ag thin films prepared by vapour [1] or DC sputter [2-4] deposition show solubility of both components (approx. 10 at.%) in each other as observed by XRD measurements. Besides of enhanced solubility formation of hexagonal (hcp) domains was also observed [4]. These results make probable the formation of metastable (ordered solid solution) phases in this system. Cu-Ag films were prepared by thermal evaporation and co-deposition of Cu and Ag at 10-5-10-6 mbar onto amorphous thin carbon foils at room temperature. The composition of the films covered a wide range of 10-60 at % of Ag. Deposition rates were around 1 nm/s. A CM20 TEM at 200 kV with a Noran EDS was used to determine the morphology, texture and chemical composition. High resolution TEM analysis was performed with a JEOL 3010 operated at 300kV. Films of eutectic composition (60 at% of Ag) are constituted of nanosized grains of slide solutions of Cu and Ag. The grain size is around a few nm as shown in the bright field and dark field images in Fig. 1. Electron diffraction patterns (Figs. 1b and 1c) show that the film has a pronounced <111> one axis texture [5]. The HREM analysis discovered the existence of domains with ordered solid solutions in the grains. Lattice fringe image of an Ag domain is shown in Fig. 2a. The FFT corresponding to the image is presented in Fig. 2b. Indexing the diffraction pattern (Fig. 2b) shows, that this crystal is oriented with its [110] direction parallel to the electron beam. The fitting of the 111 reflections (printed in italic in fig. 2b) shows the epitaxial relation between Cu and Ag crystals as evidenced by the moiré fringe in Fig. 2a. The occurrence of 100 and 110 type forbidden reflections proves that besides the enhanced solubility limit [1-4] and hexagonal ordering [4] the Cu-Ag solid solutions could arrange into ordered solid solution during the structure evolution of the film. The structure of this ordered solid solution is demonstrated in Fig. 2c obtained by Fourier filtering of Fig. 2a. These results suggest that the phase separation occurring during film growth could start by ordering processes. Ordering in solid solution can be one of the routs through the metastable states occurring between supersaturated random solid solutions and phase separated Ag and Cu grains as a final equilibrium state.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 389–390, DOI: 10.1007/978-3-540-85226-1_195, © Springer-Verlag Berlin Heidelberg 2008
390
1. 2. 3. 4. 5.
A.G. Dirks, J.J. van den Broek, P.E. Wierenga, J. Appl. Phys. 55 (1984) 4248 H.W. Sheng, G. Wilde, E. Ma, Acta Mater. 50 (2002) 475 Hao Chen, Jian-Min Zuo, Acat Materialia 55 (2007) 1617-1628 Smita Gohil, Rajarshi Banerjee, Sangita Bose and Pushan Ayyub, Scripta Materialia (2008) , doi:10.1016/j.scriptamat.2007.12.043 F. Misják, P.B. Barna, A.L. Tóth, T. Ujvári, I. Bertóti, Gy. Radnóczi, Thin Solid Films 516 (2008) 3931–3934
Figure 1. Bright field (a) and dark field (b) as well as electron diffraction patterns (c,d) of eutectic Cu-Ag film co-deposited at room temperature. The diffraction patterns reveal, the textured nature of the film in on axis ((c) and tilted (d) position.
Figure 2. High resolution image of a Ag domain (a) showing superlattice reflections of (001) and (1-10) type in the FFT pattern indicating the presence of an ordered solid solution in the Cu-Ag alloy (b). The index printed in italic in (b) is common for Cu and Ag reflections. Filtered version of the image indicating the position of the unit cell and the ordered structure in the insert (c). x stands for only Ag positions, ● stands for common positions of Ag and Cu.
391
Precipitates and magnetic domains in an annealed Co38Ni33Al29 shape memory alloy studied by TEM B. Bartova1,*, D. Schryvers1, N. Wiese2 and J.N. Chapman2 1. EMAT, University of Antwerp, Groenenborgerlaan 171, B-2020 Antwerp, Belgium 2. Department of Physics and Astronomy, University of Glasgow, Glasgow G12 8QQ, United Kingdom * now at LSME, Ecole polytechnique Fédérale, Station 12, CH-1015 Lausanne, Switzerland [email protected] Keywords: CoNiAl shape memory alloy, precipitates, magnetic domains, Lorentz microscopy
The Co-Ni-Al system undergoes a martensitic transformation from β-phase (cubic) austenite to L10 (tetragonal) martensite in a temperature range between 93 and 393 K depending on composition. Furthermore, the martensitic start temperature TMs and Curie temperature Tc can be independently controlled by the composition. TMs decreases with increasing content of Co and Al whereas Tc increases with increasing Co content and decreasing amounts of Al [1]. This work presents a detailed study of the microstructure of austenite and an investigation of the relation between magnetic and crystallographic structure. Since TMs for the material studied here is below room temperature, in-situ cooling experiments were performed involving conventional transmission electron microscopy and Lorentz microscopy. The Fresnel mode of Lorentz microscopy was used to study the magnetic domain structure of the sample. The morphology of the sample, following annealing and subsequent quenching, consists of the B2 matrix and a γ-phase. A dark field TEM image reveals small precipitates present in the B2 matrix see Fig.1. The rod-like precipitates have dimensions ranging from 10 to 60 nm for the longest axis. In the high resolution image of Fig. 2a, a single precipitate in the B2 matrix can be seen. From the fast Fourier transform (FFT) pattern it can be concluded that the B2 matrix is viewed along a [110] zone axis. The FFT of the precipitate clearly reveals hexagonal [001] or cubic <111> symmetry. The measured value d100=0.219 nm fits with the values for hcp ε-Co. Figure 2b shows the FFT pattern from the entire area of Fig. 2a. It corresponds to the Burgers orientation relationship which is in good agreement with simulation for the same case shown in Fig. 2c. In some regions close to the hole, the phase transformation is incomplete. At these positions, the habit plane between the austenite and martensite regions can be observed. In Fig. 3, a Fresnel image of such a region is shown. The magnetic domain structure has to accommodate across the interface, an inevitable consequence of the difference between the preferred domain spacing in the two phases. Moreover, in this very thin region, it is clear that there is heavy twinning within the martensite and locally the domain walls adopt irregular zig-zag structures with walls running for variable distances along either of two preferred directions. S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 391–392, DOI: 10.1007/978-3-540-85226-1_196, © Springer-Verlag Berlin Heidelberg 2008
392 1.
2.
K. Oikawa, L. Wulff, T. Iijima et al. APL 79 (20), (2001) 3290-3292 We gratefully acknowledge financial support from the MULTIMAT Marie Curie Research Training network (MRTN-CT-2004-505226).
Figure 1. (a) SEM image of the microstructure of Co38Ni33Al29 annealed alloy consisting of B2 matrix with dispersed γ-phase. (b) Dark-field image of the Co precipitates present in the B2 matrix taken from the reflection marked with a circle. (c) Diffraction pattern taken from the [110] zone axis of B2 matrix (a=0.287 nm)
Figure 2. (a) HRTEM image shows hcp precipitate in B2 matrix. (b) FFT plot taken from whole area of Fig. 2a. (c) Simulated diffraction pattern combining ε-Co precipitate along the [001] zone axis with B2 matrix in the [110] zone.
Figure 3. (a) Fresnel image of a partially transformed region of the specimen. (b) Detail close to the interface between austenite and martensite as indicated.
393
On the gallium accumulation at the boundaries of Al layers in FIB prepared TEM specimens P. Favia and H. Bender IMEC, Kapeldreef 75, 3001 Leuven, Belgium [email protected] Keywords: FIB, EDS, specimen preparation, Ga in Al
Focused ion beam milling in a dual beam FIB/SEM is nowadays the most common TEM specimen preparation method for semiconductor device structures. Numerous studies investigated the damage induced by the ion beam near the outer faces of the TEM lamellae. Methods to reduce this damage are for example low energy Ga ion milling as final milling step or low energy Ar ion milling (ex-situ or in-situ). In many materials the ion beam damage manifests itself as amorphisation of the outermost layer (e.g. ~ 23 nm in Si for 30 kV Ga). In metals the damage can result in an increase of the dislocation density [1]. An estimate of the amount of implanted Ga for different materials is discussed in [2] predicting for example the presence of 4 and 9 at % Ga in the outer <10 nm of the thinned foil for Si and W respectively. Redeposition of sputtered material will generally add more Ga on the specimens. This artefact can generally well be minimized with in-situ lift-out FIB preparation. Therefore, averaged over the specimen thickness only a minor Ga signal with weak materials dependence is to be expected in EDS analysis. Typical concentrations are reported to be in the range 0 at% [1] to < 2 at% [2]. Obviously these percentages will depend on the specimen thickness. These low Ga signals are indeed consistent with the results obtained in most of our specimens. However, a high gallium level is observed at the interface of Al layers as is illustrated on Figure 1 for an Al/SiO2/Si stack. Also in TiN/TiAl3/Al layer structures the Ga signal strongly peaks at the interfaces (Figure 2). In an early report [3] a high Ga signal observed in the TiN layer of a TiN/Al stack was attributed to the high sputtering yield of TiN. As the Ga ion beam basically mills parallel with the TEM foil, this explanation seems unlikely and more probably the lateral resolution during that measurement was insufficient to reveal that the Ga was actually peaked at the interface instead of in the TiN. The Ga accumulation at the interfaces can be understood by the rather low solubility of Ga in Al (<9at% at 26-29ºC). Grain boundary penetration of liquid Ga on Al bicrystals is extensively studied in literature [4-6] and shown to be a very fast process that can lead to embrittlement of the Al. The present observations show that this phenomenon can also occur at the interfaces of Al with other materials. 1. 2. 3.
C.R. Hutchinson, R.E. Hackenberg and G.J. Shiflet, Ultramicroscopy 94 (2003), p. 37. T. Ishitani, H. Koike, T. Yaguchi and T. Kamino, J. Vac. Sci. Technol. B 16 (1998), p. 1907. K. Park, Mat. Res. Soc. Symp. Proc. 199 (1990), p. 271.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 393–394, DOI: 10.1007/978-3-540-85226-1_197, © Springer-Verlag Berlin Heidelberg 2008
394
4. 5. 6.
R.C. Hugo and R.G. Hoagland, Scipta Materialia 41 (1999), p. 1341. W. Ludwig, E. Pereiro-Lopez and D. Bellet, Acta Materialia 53 (2005), p.151. E.E. Glickman, Z. Metallkd. 96 (2005), p. 1204.
150
Counts
Al
Si Al O Ga
100
SiO2
50
Si
a
0.0
b
50 nm
5
10 15 20 Position (nm)
25
30
Figure 1. HAADF-STEM image of the interface of a sputtered Al layer on SiO2/Si (a) and EDS line scan (b, top to bottom) across the interface showing the increase of the Ga signal near the interface of the Al and corresponding with the bright line on the STEM image. 100
SiGe
TiN
TiAl3
Al
80
TiN
Counts
SiGe
Al
Ga
60
Ti Al
40
Si Ge
20
TiAl3
a
500 nm 50 500 nm nm 500
b
50
100
150
Position (nm)
Figure 2. HAADF-STEM image of SiGe/Al contact (a) and EDS line scan (b, top to bottom) along the line indicated on the image showing the accumulation of Ga at the TiN/TiAl3 and TiAl3/Al interfaces (arrows).
395
Precipitation in an Al-Mg-Ge Alloy R. Bjorge1, C.D. Marioara2, S.J. Andersen2 and R. Holmestad1 1. Norwegian University of Science and Technology, Department of Physics, 7491 Trondheim, Norway 2. SINTEF Materials and Chemistry, 7465 Trondheim, Norway ruben.bjorge@ntnu no Keywords: precipitation, Al-Mg-Ge alloy, HRTEM, ADF-STEM
The precipitation in an Al-0.87 at% Mg-0.43 at% Ge alloy has been investigated using high-resolution transmission electron microscopy (HRTEM) and annular dark field scanning TEM (ADF-STEM). This work is a continuation of previous studies on AlMg-Si-(Cu) alloys, which are industrially relevant due to their superior mechanical properties such as high strength/weight ratio. The hardness increase is generated by the precipitation of nanometre-sized metastable phases from solid solution during artificial ageing. Most precipitates have had their crystal structures solved by our group using a combination of quantitative electron diffraction, first-principles methods and HRTEM [1-3]. It has been shown that all phases are structurally related through a near-hexagonal Si network having sub-cell dimensions a=b=0.405 nm, c=0.405 nm [3]. A possible way of improving the mechanical properties of Al-Mg-Si-(Cu) alloys is by replacing one or more solute elements with other ones having similar electrochemical properties. Total or partial replacement of Si by Ge is one such example. In bulk form Ge is similar in size to, and forms the same diamond structure as Si. An improvement in peak hardness and age-hardenability by replacing Si with Ge has previously been reported for an Al-1.0 wt% Mg2Ge alloy [4]. The higher atomic number of Ge with respect to Al and Mg makes Al-Mg-Ge alloys well suited for ADF-STEM studies. In the present work, hardness measurements indicate a moderate increase in strength and better stability during ageing for the Al-Mg-Ge alloy compared to a similar alloy containing Si instead of Ge. HRTEM and ADF-STEM images from early precipitates in the Al-Mg-Ge alloy show that Ge columns arrange in a near-hexagonal network with similar dimensions as the previously reported Si-network in Al-Mg-Si-(Cu) alloys. The Ge-network has directions parallel to <100>Al (Figure 1), producing precipitates that sometimes have plate-like morphologies. In most precipitates the atomic arrangement on the Ge-network was disordered, but a particle with a monoclinic unit cell was also found (Figure 2). This type of atomic arrangement has only been observed in the AlMg-Si-Cu alloys [5]. 1. 2. 3. 4. 5.
S. J. Andersen et al., Materials Science and Engineering A 390 (2005), p. 127. R. Vissers, et al., Acta Materialia 55 (2007), p. 3815. S. J. Andersen et al., Materials Science and Engineering A 444 (2007), p. 157. K. Matsuda, S. Ikeno and T. Munekata, Materials Science Forum 519-521 (2006), p. 221. C. D. Marioara et al., Philosophical Magazine 87 (2007), p. 3385.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 395–396, DOI: 10.1007/978-3-540-85226-1_198, © Springer-Verlag Berlin Heidelberg 2008
396
Figure 1. Fourier-filtered ADF-STEM images of early-stage precipitates in the Al-MgGe alloy with the matrix in a <100>Al orientation. The image shows that the Ge columns are arranged in a near-hexagonal configuration with sub-cell dimensions a=b=0.405 nm, c=0.405 nm. The sub-cells are oriented parallel to <100>Al directions. This atomic arrangement is very similar to what has been found in the Al-Mg-Si-Cu system [5].
Figure 2. HRTEM image and corresponding FFT of a plate-like precipitate in the AlMg-Ge alloy viewed along <100>Al. Although the precipitate is partly disordered, a monoclinic unit cell of dimensions a=1.215 nm, b=1.032 nm, c=0.405 nm, γ=101.3° can be observed. The unit cell is also a super-cell in Al, as indicated.
397
Interaction between dislocations and oxide precipitates in an aluminium containing ferritic stainless steel L. Boulanger, S. Poissonnet and F. Legendre Commissariat à l'Energie Atomique, DEN/DANS/DMN Service de Recherches de Métallurgie Physique Centre d'Etudes de Saclay, F91191 Gif-sur-Yvette, France loic.boulanger@cea fr Keywords: precipitates, dislocations, strain contrast
Ferritic and martensitic steels strengthened by oxide dispersion (ODS) are studied at the nanometre scale because the interaction between dislocations and nanosized precipitates drives mechanical behaviour and evolution during neutron irradiation. Observation by Analytical Electron Microscopy (AEM) aside chemical information brings information about the coherency of precipitates, their strain field and the surrounding dislocations. We investigated the PM2000 alloy (Fe-19Cr-5.5Al-0.5Ti-0.5Y203 (wt.)) manufactured by Plansee. It contains a large range of precipitates which can be classified into two groups: respectively around 5 nm and 50 nm. The smaller contain Al-Y-O (1]. Our purpose is to show the contrast of nanoprecipitates under two beam imaging and their association to the dislocations. Two metallurgical states have been investigated, the asreceived state and an in-situ annealed obtained by heating inside the electron microscope at 930°C during 3 mn. In the as received material two dark lobes contrast “Figure 1”, so-called AshbyBrown contrast [2], is clearly visible on bright field images. Histograms sizes on out of contrast images give the same distribution. Among them, larger precipitates (> 10 nm) present parallel fine fringes attributed to moiré patterns “Figure 2”. An image compatible with a screw dislocation (b= ½[-1, -1, 1]) is visible on figure 1. Images realised with two perpendicular reflections of type (110) show a rotation of the lobes position “Figure 3a and 3b”. After in-situ annealing few evolutions is present: dislocations are still pinned on precipitates “Figure 4”. They show the very same strain contrast but sometime their square shape is better resolved. As conclusion, PM 2000 alloy contains very small precipitates (3 nm) clearly seen under two beams imaging. A dark contrast line is present that is aligned with the reflection vector according to a spherical strain. Above 7 nm moiré contrasts are present likely due to a relaxation of the stress. This structure is thermally stable up to 930°C. 1 2
M. Klimiankou, R. Lindau, A. Möslang and J. Schröder, Powder Met. 48(2005), p. 277. M. F. Ashby and L. M. Brown, Philos. Mag. 8(1963), p. 1649.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 397–398, DOI: 10.1007/978-3-540-85226-1_199, © Springer-Verlag Berlin Heidelberg 2008
398
Figure 1. Two beams image
Figure 3a. First reflection: double lobes and dislocation line
Figure 2. Double lobes and moiré patterns
Figure 3b. Perpendicular reflection: rotation of lobes, the dislocation image vanishes
Figure 4. After annealing, the square shape becomes more visible
399
Voids Associated with Nano-Particles of Tin in Aluminium Laure Bourgeois1,2, Matthew Weyland1 and Barry C. Muddle2 1. Monash Centre for Electron Microscopy, Monash University, VIC 3800, Australia 2. Centre of Excellence for Design in Light Metals, Monash University, VIC 3800, Australia Department of Materials Engineering, Monash University, VIC 3800, Australia [email protected] Keywords: vacancy clusters, aluminium alloy, transmission electron microscopy
Vacancies play a crucial role in many aluminium alloys: they mediate the diffusion of most solute atoms, relieve the compressive strain of precipitates, and must be present above a critical concentration for certain phases to nucleate [1]. Unfortunately vacancies and their association to solute atoms or precipitates can only be detected indirectly. In this work, transmission electron microscopy (TEM) is used to show that under certain circumstances three-dimensional objects containing a large amount of vacancies form in association with tin precipitates in aluminium. These objects bear some similarities to voids observed in other systems [2-3]. The examined samples were alloys of Al-0.01at%Sn and Al-1.7at%Cu-0.01at%Sn; these are model alloys for the study of micro-alloying additions (Sn in this case) on the precipitation behaviour of Cu-rich phases [4-5]. The samples were heat treated according to the usual regimes for precipitation-hardened aluminium alloys, with ageing temperatures ranging between 350 and 485°C. The TEM observations were performed on a JEOL 2011 operating at 200 kV. Figure 1(a) shows a bright-field image of a small cluster of tin particles observed in the Al-0.01Sn alloy. Each particle exhibits a single spheroidal region (see arrows) of contrast lighter than the dark tin particle. Figure 1(b) shows a lattice image of another such case. Energy dispersive x-ray (EDX) spectra collected with a focused 5 nm probe on different regions of the group shown in Figure 1(b) are presented in Figure 1(c). No elements other than aluminium or tin were found associated with the “bubble” contrast (the copper peak is an artefact). In particular, no enrichment in oxygen or other volatile element was detected. Examination of the diffraction contrast due to the “bubble” features over an extensive range of specimen holder tilts failed to detect any crystalline phases other than aluminium and copper. Furthermore, several examples were found of broken shells at the surface of tin particles, suggesting that the “bubbles” are empty. Further confirmation that these objects are either empty or at least contain significant amounts of vacancies was provided by the nature of the Fresnel fringe contrast at the matrix-void interface. Figure 2 shows the change in the Fresnel fringe at the matrix-void interface as a function of objective defocus. The fact that the white fringe faces the “bubble” region at the negative focus condition, and the matrix in the positive focus condition, is a clear indication of a lower projected charge density at the “bubble” region. These objects can therefore be regarded as voids. S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 399–400, DOI: 10.1007/978-3-540-85226-1_200, © Springer-Verlag Berlin Heidelberg 2008
400
In the Al-0.01Sn alloy only a relatively small number of tin particles were observed associated with voids, and this only occurred at the high ageing temperature of 445°C, which is slightly less than the temperature where liquid tin dissolves into the matrix (460°C; note that the bulk melting point of tin is 232°C). However in the Cu-containing Al-1.7Cu-0.01Sn alloy, the voids were more common and persisted along with the tin particles well above the tin solvus in pure aluminium; the voids were often found at the triple junction of tin, aluminium, and a copper-rich grain. Sn is known to have a high vacancy binding energy. It is therefore not altogether surprising to find Sn particles associated with vacancy clusters. A possible mechanism might involve the nucleation of voids in the vacancy-supersaturated region surrounding a tin particle, the excess vacancies being liberated from solute tin atoms incorporated into the growing precipitate. The fact that the voids are often seen attached to a smaller grain on the surface of the tin particles suggests that they nucleate heterogeneously. 1. 2. 3. 4. 5.
K.C. Russell, Scripta Metallurgica 3 (1969), p. 313. C. Cawthorne and E.J. Fulton, Nature 216 (1967), p. 575. J.S. Williams, M.J. Conway, B.C. Williams and J. Wong-Leung 78 (2001), p. 2867. H.K. Hardy, J. Inst. Metals 80 (1951-52), p. 483. L. Bourgeois, J.F. Nie and B.C. Muddle, Philos. Mag. 85 (2005), p. 3487.
(a)
(b)
(c)
Figure 1. (a) Tin particles in Al-0.01Sn associated with spheroidal contrasts interpreted to be voids (see arrows); (b) lattice image of a tin-void group taken along the [100] zone axis of aluminium; (c) EDX spectra taken with a focused 5 nm probe for the different components of the group shown in (b).
Δf=-540nm
Δf=-72nm
Δf=+384nm
20 nm Figure 2. Part of a through-focal series, from underfocus (left) to overfocus (right). The Fresnel fringe contrast at the matrix-void interface as a function of objective defocus Δf confirms that the void region has a projected charge density that is less than the aluminium matrix and must therefore contain vacancies.
401
Influence of thermal treatments in microstructure and recrystallization peak energy of P/M Al-Mg-X alloys S.J. Buso1,2, A. Almeida Filho1, I.M. Espósito1,2, J.R. Matos4, W.A. Monteiro2,3 1. Centro Universitário Sant’Anna – São Paulo - Brazil 2. Instituto de Pesquisas Energéticas e Nucleares IPEN/USP– São Paulo - Brazil 3. Universidade Presbiteriana Mackenzie – São Paulo - Brazil 4. Instituto de Química da Universidade de São Paulo IQ/USP– São Paulo – Brazil [email protected] Keywords: Aluminum Alloys, Thermal Analysis, Electron Microscopy, Recrystallization
Light materials have been studied thoroughly and used in components of pieces in the automobile, naval and aerospace industries in the last decade. Among those materials, the aluminium-magnesium alloys have special attention due, not only to the lightness of the material, but also to certain mechanical properties and reciclability[1,2]. In this work, samples of Al-2Mg-1Nb and Al-2Mg-0.6Zr alloys were produced, by powder metallurgy techniques, employing uniaxial hot compactation (400 MPa) and extrusion (60 MPa) both processes at 450oC. The product of these processes were bars of ∅ = 15 mm and length of 200 mm. The bars of the alloys were cold worked, without intermediate thermal treatments in a rolling mill being obtained reduction in area of 80%. Samples of both alloys in study were analyzed, without previous thermal treatments, at DSC in equipment SHIMADZU DSC 50 of the Laboratory of Thermal Analyses of the IQ/USP. From the same alloys lot, were prepared samples for TEM analysis in microscope JEM200C of the IPEN/USP. The figures 1.a and 1.b show the sequences of the analyses of DSC in samples of Al-2Mg-0.6Zr and Al-2Mg-1Nb alloys in temperature range between 400oC and 550oC, the curves shows the peak of the initial recrystallization energy for the alloys in study. The figures 2 to 3 show the microstructure observed by TEM of the samples in study. In the analyses of samples of Al-2Mg-0.6Zr and Al-2Mg-1Nb alloy, grains are observed with possible precipitates close to grain boundaries and inside the grains, in the samples without thermal treatment (figures 2.a and 3.a). After 60s of thermal treatment at 550oC (figures 2.b and 3.b) a distribution of precipitates and a strong interaction between dislocations and precipitates are observed. These processes are characteristic of the recovery and recrystallization. 1. 2.
Buso, S. J.; Monteiro, W. A. Microstructural characterisation of a P/M Al-Mg-Zr alloy after thermal treatmensts. Acta Microscópica, v. 9, p. 153-154, 2000. Buso, S. J., Monteiro, W. A.. Characterisation by TEM of a supersatured P/M Al-Mg-Zr alloy after thermal treatments In: International Conference on Processing & Manufacturing of Advanced Materials (Thermec’2003), 2003, Madrid, Proccedings of the International Conference on Processing & Manufacturing of Advanced Materials, 2003.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 401–402, DOI: 10.1007/978-3-540-85226-1_201, © Springer-Verlag Berlin Heidelberg 2008
402
(a)
(b)
Figure 1. Sequences of the analyses of DSC in samples of: a)Al-2Mg-0.6Zr and
b) Al-2Mg-1Nb
(a)
(b)
Figure 2. Micrographies of samples of Al-2Mg-0.6Zr: a) without thermal treatment and
b) 60s, 550oC
(a)
(b)
Figure 3. Micrographies of samples of Al-2Mg-1Nb: a) without thermal treatment and b)
60s, 550oC
403
Analytical TEM of Nb3Sn Multifilament Superconductor Wires M. Cantoni1, V. Abächerli2, D. Uglietti2, B. Seeber2 and R. Flükiger2 1. EPFL-CIME, Bat. MXC-134, Station 12, CH-1015 Lausanne 2. Group of Applied Physics, University of Geneva, CH-1211 Geneva [email protected] Keywords: TEM, EDX, FIB
Bronze processed Nb3Sn superconducting wires are today still considered as the best candidates for nuclear magnetic resonance (NMR) magnets operating in persistent mode at high magnetic fields. The metallurgical treatment of Nb3Sn bronze wires with additives like Ta and Ti is quite difficult to further improve because the correlation between the additive and its effect on the superconducting properties, which do not only depend on its concentration but also on the whole variety of fabrication parameters. The aim of this work is to clear up the different effects of the internal (Nb-Ta / Nb-Ti filaments) and external (Cu-Sn-Ti bronze) Ti doping method on the superconducting properties and to analyze their possible reasons [1]. Conventional techniques of specimen preparation did not lead to TEM-samples with the required large and thin areas for the analysis because of severe preferential thinning of the bronze matrix around the Nb3Sn filaments. The focused ion beam (FIB) was used to cut out lamellae of 20x5um size directly from a cable, to attach them to a TEM grid and to thin them further to electron transparency (Fig. 1a). The samples obtained this way have uniform thickness and are ideally suited for EDX-Analysis and elmental mapping. Already the raw intensitiy maps of the elemental distribution (Fig. 1b) allow an interpretation of concentration gradients. Transverse as well as longitudinal crosssections permitted the investigation of the grain structure and the elemental distribution parallel and perpendicular to the cable’s axis. Scanning Transmission Electron Microscopy (STEM) in combination with Energy Dispersive X-Ray (EDX) Microanalysis was used to analyze the chemical composition of the superconducting phase. A gradient of Sn was found across the individual filaments reducing this way the overall “useful” superconducting cross-section in high magnetic fields. EDX as well as energy filtered imaging (EFTEM) were used to investigate and trace the additives on a nanometer scale at the grain boundaries (Fig. 2). Cu could be found in almost all the grain boundaries where as the Ti was only present at the grain boundaries when the internal Ti doping method was applied. This finding allows to engineer grain boundaries and to control the superconducting properties of these multi-filament cables. 1. 2.
Abächerli V, Uglietti D, Seeber B, Flükiger R, Physica C 372-376 (2002), 1325-1328. We kindly acknowledge EPFL-CMI for the access to the FIB.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 403–404, DOI: 10.1007/978-3-540-85226-1_202, © Springer-Verlag Berlin Heidelberg 2008
404
Figure 1. left) STEM dark field image: cross-section of a single superconductor filament. The inset shows the TEM lamella prepared by FIB. right) EDX element maps (raw intensity of selected x-ray peaks) of Nb and Sn. The remaining un-reacted Nb core and a gradient in the Sn concentration are clearly recognizable.
Figure 2. a) STEM dark field image (left) with EDX linescan (arrow). The linescan profiles (right) of Cu-L and Ti-K peaks show an increased concentration of Cu and Ti at the grain boundary.
405
3D Reconstruction of Ni4Ti3 Precipitates in Ni-Ti by FIB/SEM Slice-and-View S. Cao, W. Tirry, W. Van Den Broek and D. Schryvers EMAT, University of Antwerp, Groenenborgerlaan 171, B-2020, Antwerp, Belgium [email protected] Keywords: Ni4Ti3, 3D reconstruction, FIB/SEM
Ni4Ti3 precipitates with lenticular shape and rhombohedral atomic structure growing in the austenitic B2 matrix of binary Ni-rich Ni-Ti alloys upon proper annealing treatment have an important influence on the shape memory effect which originates from the martensitic transformation of B2-B19’ [1]. Figure 1 shows a typical 2D distribution of such precipitates as obtained by TEM under conventional imaging conditions. A slice-and-view procedure in a Dual-Beam FIB/SEM system has been applied to investigate the 3D distribution and morphology of these precipitates, in order to indicate their influence in the martensitic transformation. A bulk of material has been sliced away step by step using the Ga+ ion beam, and for each slice a 2D SE image has been taken. In this preliminary experimental setup the step size used is 100nm with a total of 55 steps, leading to an investigated volume of 136µm3. Due to the weak contrast of the precipitates, proper imaging conditions need to be selected to allow for semi-automated image treatment and an optimization procedure to find those has been followed. One of the SE images obtained from the Dual-Beam is shown is Figure 2(a)), proper alignment and image processing in MatLab© [2] and Amira© [3] are performed on the whole sequence to create a sequence of binary images (as one is shown in Figure 2(b)). A 3D reconstruction has been achieved via these 2D binary images (shown in Figure 3(c)), from which both qualitative and quantitative analysis can be performed. Finally, a volume ratio of 10.2% for the Ni4Ti3 precipitates could be calculated, summed over all variants, which yields a net composition of Ni50 27Ti49 73 for the matrix, leading to an increase of 125 degrees for the martensitic start temperature Ms. Also, the orientation between two precipitates could be measured as an average angle of 109.4° ± 1.1°, which confirms the relative orientation of the different variants of the precipitates between {111} family planes in theory (109.5°). The present work thus indicates that slice-andview is a valuable tool for the investigation of the 3D distribution and related parameters of technologically important precipitates in alloys such as Ni-Ti. In the near future, other quantitative measures on the distribution of the precipitates will be obtained. 1. 2. 3.
K. Otsuka, X. Ren, Progress in Materials Science 50 (2005), p. 511 Information on http://www mathworks.com/products/matlab/
Information on http://www.amiravis.com/
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 405–406, DOI: 10.1007/978-3-540-85226-1_203, © Springer-Verlag Berlin Heidelberg 2008
406
4.
We kindly acknowledge the help of MULTIMAT “Multi-scale modeling and characterisation for phase transformations in advanced materials”, a Marie Curie Research Training Network (MRTN-CT-2004-505226) of the European Commission for supporting this work.
Figure 1. Schematic drawing of the lens-shaped Ni4Ti3 in the two zones: (a) the [1 0 1]B2; (b) the [1 1 1]B2; (c) Typical TEM BF image showing four variants of Ni4Ti3 precipitates
Figure 2. One of the 2D cross-section images before (a) and after (b) background subtraction, and 3D reconstruction for all the Ni4Ti3 precipitates (c)
407
Electron microscopy study of Mg78.5Pd21.5: a phase with nanothin 120° rotational twin domains W. Carrillo-Cabrera, J.P.A. Makongo, Yu. Prots, G. Kreiner Max-Planck-Institut für Chemische Physik fester Stoffe carrillo@cpfs mpg.de Keywords: Mg78 5Pd21 5, rotational twinning, TEM study
Complex intermetallic alloy phases are intermetallic compounds with giant unit cells. They have a preference to accumulate at specific compositions. Therefore, it is difficult to obtain single phase materials and to determine their crystal structures. An example is “Mg4Pd”, first reported by Ferro [1]. No crystallographic data was known until Spiekermann [2] reported the large orthorhombic structure of Mg306Pd77 (Mg3 97Pd). In a study to find out the phase equilibria in the Mg-rich part of the Mg-Pd system [3] we additionally obtained three phases close to the composition Mg4Pd: Mg78 5Pd21 5 (Mg3 65Pd), Mg56 4Pd13 5 (Mg4 18Pd) and Mg57Pd13 (Mg4 38Pd). Our aim in this contribution is to demonstrate typical problems arising during the crystal structure determination of complex metallic alloy phases using Mg78 5Pd21 5 as an example. Its complex X-ray powder pattern (CuKα1) can be indexed on the basis of a hexagonal unit cell (ah = 28.046(8) Å, ch = 27.950(4) Å). A preliminary structure model was refined using single crystal X-ray data (Rint = 12.1%; wR2 = 29.3%, R1 = 16.4%). The calculated profile using this hexagonal model fits roughly the observed X-ray powder pattern (RB = 8.8%; wRp = 6.4%). However, this hexagonal model shows anomalous disordering features. Subsequent electron micrographs (Figures 1) clearly show that a “single crystal” specimen in reality consists of an intergrowth of narrow twinned planar domains parallel to the (001)h plane, which explains the hexagonal model inconsistencies. Further analysis demonstrated that the crystal structure is orthorhombic (a = 48.5729(9) Å, b = 28.0532(4) Å, c = 27.9859(5) Å, space group Fmmm) and the nanothin (5−50 nm) domains are 120° rotational twins oriented in three different directions perpendicular to the c-axis (Figure 2). FIB cuttings perpendicular and parallel to the c-axis were indispensable for this study. A more detailed study of the crystal structure and micro-structure of Mg78 5Pd21 5 (XRD, SAED, TEM, HRTEM) will be presented. 1. 2. 3. 4.
R. Ferro, J. Less-Common Met. 1 (1959), 424. S. Spiekermann, Doctoral Thesis, University Dortmund (1998). J. P. A. Makongo, Y. Prots, U. Burkhard, R. Niewa, C. Kudla. G. Kreiner, Phil. Mag. 86 (2006), 3. Part of this work has been done at the Special Electron Microscopy Laboratory at Triebenberg, Technical University of Dresden. We thank Prof. H. Lichte for his support.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 407–408, DOI: 10.1007/978-3-540-85226-1_204, © Springer-Verlag Berlin Heidelberg 2008
408
[001] [001
001 1
2
2
3
1
2
3
Figure 1. TEM images of Mg78 5Pd21 5, showing nanothin domains (5−50 nm thick) perpendicular to the c axis. (left) overview, FIB cut parallel to the c axis. (right) Middle resolution TEM image of crushed particle, the layered domains are labelled as 1, 3 (viewed along [110]) or 2 (marked with arrows, viewed along [010]).
a 3* 3 2
220 000
1
b 3*
[001] Figure 2. Selected area diffraction patterns of Mg78 5Pd21 5 along [001]. FIB cut perpendicular to the c axis. (left) SAD of thick region with overlapped domains (1, 2, 3) and (right) SAD of one-domain region.
409
Analysing small precipitates in a ferritic steel matrix A.J. Craven and M. MacKenzie Dept. Physics & Astronomy, University of Glasgow, Glasgow, G12 8QQ, UK [email protected] Keywords: electron energy loss spectroscopy, spectrum imaging, precipitates, steel
The strength of a microalloyed high strength low alloy steel is controlled by a number of factors including the grain size and the fine dispersion hardening precipitates. For sheet steel, the latter form after the final rolling pass, during and following the austenite to ferrite phase transformation. The majority of these particles are sub-10nm. Both 3 dimensional atom probe (3-DAP) and spectrum imaging (SI) using electron energy loss spectroscopy (EELS) have shown the peak in the size distribution in a Vbased steel is around 2nm [1]. As well as the size distribution, the composition of the particles is also of great interest. Earlier work using extraction replicas had shown that particles above 4nm in size were essentially nitrogen rich carbonitrides but there was some uncertainty as to whether a plasma process, used to thin the support film, was modifying the composition [2]. The more recent work, using both 3-DAP and EELS SI to analyse the particles within the ferritic matrix, confirmed that these results also applied to particles below 4nm in size [1]. 3-DAP had difficulty in quantifying the N content while confirming the low C content. In fact, the C seemed to form an “atmosphere” around the particles rather than being contained within them. SI was able to quantify the N but had difficulty determining the C content because of a perturbation of the background shape in front of the C K-edge. This perturbation is a major problem since its features are much bigger than the C K-edge intensity from a small particle. To avoid upsetting the objective lens with a large amount of ferromagnetic material, the specimen for EELS SI was made by focused ion beam lift out using 30keV Ga ions. The surface damage was removed using subsequent broad beam ion milling at 500eV. SI was carried out with a probe of half-angle 13mrad containing 0.19nA and using a collection half-angle of 27mrad and 1eV/channel. Figure 1 shows the residual shape left after spectra from the matrix had the background removed using a power law background model fitted in the region from 230 to 280eV. The spectra were recorded at different positions on the detector array and have been normalised to the first peak. Since the energies of the features are independent of the position on the detector, the perturbation arises from the matrix. It is ~2.5% of the background before the C K-edge. A method of modelling and accurately removing this perturbation is required. Since the particles are small and well separated, the surrounding matrix should provide a good model of the background. The particle positions are easily identified by mapping the intensity of the V L2,3 white lines. Thus the spectra in the pixels corresponding to the particles can be summed. If the size of the summed region over the particle is increased, the additional signal is purely matrix and this matrix contribution can be isolated by subtracting the sum obtained from the smaller region. Thus spectra from the particle plus matrix and the matrix alone can be obtained.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 409–410, DOI: 10.1007/978-3-540-85226-1_205, © Springer-Verlag Berlin Heidelberg 2008
410
Since the perturbation comes from the matrix, which is essentially Fe, the two spectra are normalised by the counts in the corresponding regions of an Fe L2,3 map. Figure 2 shows two such normalised spectra while Figure 3 is their difference. This difference is just the spectrum from the particle itself and is only ~1% of the total signal cf 2.5% for the background perturbation. While the difference is noisy, it is clear there is little intensity from the C K-edge but significant intensity from the N K-, V L2,3- and Mn L2,3-edges. The intensity from the Fe L2,3-edges has gone but there is some differentiation of the white lines due to jitter on the accelerating voltage. Similarly the O K-edge signal from the surface oxidation has been removed. Figure 4 shows the sum of the spectra extracted from 5 particles and compares it to spectra from stoichiometric VC and VN standards. These have been scaled to have the same intensities over the energy range 510 to 620eV. It is clear that the C content in the particles is low or nonexistent while the N content is close to that of stoichiometric VN. Thus EELS SI has the ability to analyse particles in the sub-4nm size range within a steel matrix but care must be taken with the processing of the data. 1. 2.
A.J. Craven, M. MacKenzie, A. Cerezo, T. Godfrey and P.H. Clifton, Mat. Sci. Tech. in press. J.A. Wilson, A.J. Craven, Y. Li and T.N. Baker, Mat. Sci. Tech. 23 (2007) 519. 1E +6
3 E +6 En e rg y Lo s s ( e V) 230
330
430
Electrons
Electrons
0 E +0 530
- 1E +6
2 E +6
1E +6
- 2 E +6
0 E +0 200
- 3 E +6
Figure 1. Residuals left after power law background subtraction fitted over 230 – 280eV.
800
Figure 2. Spectrum from particle plus matrix (thin black) and matrix (thick grey)
3 E+4
4E+4 3E+4 Electrons
2 E+4 Elect ron s
400 600 E n e rg y Lo s s ( e V)
1E+4
2E+4 1E+4 0E+0
0 E+0 20 0
40 0 60 0 E ne rg y Lo s s ( e V)
80 0
2 00 -1E+4
400 600 Ene rg y Lo s s (eV)
800
Figure 3. The difference between the spectra in Figure 4. Background subtracted sum of spectra Figure 2. 1% of the signal is from the particle. from four particles compared to VC and VN.
411
Failure analysis of first stage land-based gas turbine blades F. Delabrouille1, F. Arnoldi1, L. Legras1 and C. Cossange1 1. EDF R&D Les renardières, department MMC, 77818 Moret sur Loing, France Frederic.delabrouille@edf fr Keywords: superalloy, crack, Inconel 738LC
The failure of a Gas Turbine (GT) first stage blade was investigated by visual inspection, scanning electron microscopy, electron probe microanalyser and transmission electron microscopy. The objective of this studies is to characterize and identify the microstructural changes involved in this failure. In order to carry out examinations and analyses, sections of the airfoil were cut using spark machining at half-height of blade. The blade was characterized using a LEO SUPRA 35 SEM. A TECNAI F20 operating at 200 kV is used for all TEM imaging. The macrostructure examinations show a lot of grains in the blade wall. The grains have a lengthened shape near the surface and is relatively equiaxe inside. This blade was made of the widely used Ni-base superalloy Inconel 738LC. Inconel 738LC have a typical superalloy microstructure, it’s a multiphase microstructure consisting of γ matrix, bimodal γ’ precipitates, γ-γ’ eutectics, interdendritic MC and M23C6 carbides. Two main zones of damage were observed : two cracks on the airfoil tip and one crack on pressure side near platform cooling hole. The examinations was carried out on one crack on the airfoil tip. The cross-section examinations show that the crack are initiated at the interface between thermal barrier coating and bond coat located under spallation zones. The crack growth was mainly interdendritic, with some transgranular zones (Figure 1). When the crack is interdendritic the matrix is not deformed, the deformation is only observed in the zones where the crack is transgranular (Figure 2). The metallographic examinations were completed by detailed observations of the crack tip using transmission electron microscopy. The crack tip is located in a MC carbide (Figure 3) . The crack changes of direction at the carbide / metal interface and restart perpendicularly in the primary carbide. The crack propagates along crystallographic steps about 10 nanometres to form an arch of circle up to the crack tip. The width of the crack is about 200 nm at the level of the observed zone. The EDX analysis didn’t show significant enrichment in oxygen on the crack lips and no variation of the contents of elements of the alloy. The mixed character of propagation, the absence of creep cavities and the presence of fine striations in initiation zone let suppose that thermo mechanical fatigue is the main mechanism responsible of cracking. The absence of oxide at the crack tip implies that the crack propagation is due to thermomechanical loading at low temperature. The current work indicates that the mechanism seems to be the out of phase thermomechanical fatigue. However, it’s not possible to eliminate totally a secondary influence of creep and high cycle fatigue.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 411–412, DOI: 10.1007/978-3-540-85226-1_206, © Springer-Verlag Berlin Heidelberg 2008
412
Figure 1. Cross-section examination of crack at airfoil tip (SEM, backscatter detector).
Figure 2. Orientation map near the crack tip at the airfoil tip.
Alloy
Crack tip
Carbide Figure 3. Bright field image of the crack tip at the level of a primary carbide.
413
TEM investigation of microstructures in low-hysteresis Ti50Ni50-xPdx alloys with special lattice parameters R. Delville1, D. Schryvers1, Z. Zhang2, S. Kasinathan2, R.D. James2 1. Electron Microscopy for Materials Science (EMAT), University of Antwerp, Groenenborgerlaan 171, B-2020 Antwerp, Belgium 2. Department of Aerospace Engineering and Mechanics, University of Minnesota, Minneapolis, Minnesota 55455, USA [email protected] Keywords: shape-memory alloy, low hysteresis, twinning
NiTi is one of the most popular shape-memory alloys (SMA) in medical applications because of its biocompatibility and its remarkable properties that allow recoverable mechanical energy to be stored in a compact delivery system. Still, its undesirable fatigue properties exemplified by the occurrence of medical-device fracture, along with large temperature/stress hysteresis and the narrow temperature range of operation translate to a tight margin of error for engineering design of the devices. A new theory on the origin of reversibility of phase transformations predicts the microstructures and explains the fundamental cause of large transformation hysteresis commonly shown by SMAs [1]. It predicts that the hysteresis can be drastically minimized by improving the geometric compatibility of the martensite and the austenite. This has been demonstrated [2] with alloys with special lattice parameters with a middle eigenvalue of their transformation matrix satisfying λ2=1 [2,3,4]. Their hysteresis decreases as the middle eigenvalue gets closer to one. The present work focuses on the TEM investigation of ternary Ti50Ni50-xPdx alloys in which different amounts of Pd substitution on Ni lead to special ratios between the austenite and martensite lattice parameters. As the compatibility between the two phases increases, a change in the microstructure is observed. Away from the compatibility condition with λ2>1, martensite plates contain fine internal twins (microtwins) which are the result of stress accommodation at the austenite-martensite habit plane. Electron diffraction shows that the fine twinning occurs along a (1-11) type I mode. Martensite plates are also found to be related to each other along a <2-11> type II twinning mode. Calculations derived from the Geometrically Non-Linear theory of Martensite (GNLTM) [1] predict the two observed twins along with a (011) compound twin. It can also be demonstrated theoretically that as λ2>1, compound twins are forbidden. Conversely, as λ2<1, type I/II twins are forbidden and only compound twins allowed. As the content of Pd is decreased toward the compatibility condition, detwinning of the martensite is observed. When the compatibility condition is satisfied (Ti50Ni39Pd11) the microstructure contains large plates of untwined martensite (figure 1). Internal microtwins have completely disappeared. Since the distortion is minimal, twins do not need to be fine. Random twinning is observed, contrasting with ordered stacks of twins observed with alloys away from the compatibility condition. Twinning seems to occur
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 413–414, DOI: 10.1007/978-3-540-85226-1_207, © Springer-Verlag Berlin Heidelberg 2008
414
along boundaries of martensite plates or as a result of nucleation variation. In addition to the (1-11) type I and <2-11> type II twins, (011) compound twins are also observed. This can be accounted to the fact that the sample sits at the limit condition λ2=1, thus allowing the three type of twins to coexist in the sample due to local lattice parameters variation. An ongoing study of local variation of composition (EDS, EELS) or lattice parameters (CBED) is attempting to relate them to the type of twins. In-situ study of the growth of martensite inside the austenite is made possible at the Ti50Ni40Pd10 composition which contains nucleated martensite inside the austenite at room-temperature. Preliminary results show exact austenite-martensite habit planes with no traces of twinning. It agrees with the fact that Ti50Ni40Pd10 is also very close to satisfying the compatibility condition. In-situ cooling will show how such a twinless martensite can grow along the habit plane and how the final martensite microstructure arises. 1. 2. 3. 4. 5.
Ball, J. M., James R.D., Phil. Trans. R. Soc. Lond., (1992) A 338-339. J. Cui et al., Nature Materials 5 (2006) 286-290. K.A. Bywater, J.W. Christian, Phil. Mag. 25-26 (1972) 1249-1273. W.J. Moberly, J.L. Proft, T.W. Duerig, R. Sinclair, Mat. Sci. For., 56-58 (1990) 605-610. We kindly acknowledge the support from the Marie Curie Research Training Network MULTIMAT “Multi-scale modelling and characterization for phase transformations in advanced material” (MRTN-CT-2004-505226)
Figure 1. Change of microstructure with composition is shown in the bright field images (a)-(c). Fig. (a) shows internally twinned martensite plates, (b) shows the detwinning of the plates and (c) a twinless plate when the compatibility condition is satisfied. SAD patterns (d,e) correspond to plates A and B in (a), respectively, showing a (1-11) type I twinning. SAD pattern (f) was taken over the twin boundary C and shows a <2-11> type II twin.
415
Evidence of silica layer at the interface between ferrite and the chromium oxide scale in oxidized Fe-Cr-Si alloys G. Bamba , P. Donnadieu, Y. Wouters and A. Galerie SIMAP, INPGrenoble-CNRS-UJF, BP 75, 38402 Saint Martin d'Hères – France [email protected] Keywords: TEM, stainless steels, oxidation, silica, adhesion
The kinetic law of oxidation of Fe-Cr-Si ferritic steels strongly depends on the Si content [1]. In addition, the chromia scale formed during oxidation exhibits strong spallation on cooling function of oxide thickness but no spallation for Si-free alloy, up to a scale thickness of 2.7 μm. Such observations are usually attributed to the presence of silica formed at the steel-chromia interface, modifying both oxidation kinetics and scale-metal adhesion [2]. Though a continuous silica layer is frequently invoked as an explanation for enhanced spallation, mainly in austenitic stainless steels, few morphological details of this layer have been produced. A series of Fe-15Cr-Si ferritic stainless steels, containing 0, 0.5 and 1 wt.% Si, were oxidized in different atmospheres between 850°C and 950°C. In all cases, SEM investigations were unable to evidence details at the interface between the chromia scale and ferrite. TEM has been then carried out on two Fe-15Cr-Si alloys which have been oxidized at 850°C under two different atmospheres : 150 mbar H2O for 72h (sample 1), 150mbar O2 for 24 h (sample 2). Cross section samples suitable for TEM observations of the oxide layers have been prepared by the FIB technique. In sample 1 (Fig. 1), a continuous layer of silica is detected, as attested by the diffraction pattern taken in this area (Fig. 1b) and the composition measured by EDX (Fig. 1c). This silica layer is about 0.5 μm thick and displays a regular shape (Fig. 1d). In some places, the silica layer grows more deeply inside the ferrite grains. The chromia scale is formed by small grains (about 0.1 μm). It is worth noting that the silica layer is separated from the chromia scale by small ferrite grains. Figure 2 shows the FIB section and the interfacial area in sample 2. A silica layer is observed, but it is discontinuous and much thinner (about 50 nm) than in sample 1. The chromia scale is still formed by a fine grain microstructure. As illustrated here, a TEM study of FIB cross section can easily evidence the silica layer formed during oxidation even for very thin layers. Preparing the section with the FIB technique was essential because of the brittleness of the interface which prevents from using classical methods. TEM gives also a measurement of the silica layer as well as the chromia scale which are usually estimated indirectly by thermogravimetric analysis. This TEM investigation points out the different behaviour of the alloys in terms of silica layer formation such information should be particularly important for the understanding of the oxidation mechanism and of the spallation effect. 1. 2.
G. Bamba, Y. Wouters, A. Galerie, F. Charlot, A. Dellali, Acta Mater. 54 (2006) p. 3917. H.E. Evans, D.A. Hilton, R.A. Holm, S.J. Webster Oxid Met 19 (1983) p. 1.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 415–416, DOI: 10.1007/978-3-540-85226-1_208, © Springer-Verlag Berlin Heidelberg 2008
416
Chromia scale
Silica layer
Silica layer ferrite
Figure 1. TEM image of the interfacial area observed in the FIB cross section from sample 1 (Fig. 1a), electron diffraction pattern (Fig. 1b) and EDX spectra (Fig. 1c) taken in white layer area in Fig. 1a. High magnification image of the silica layer (Fig. 1d) and of the chromia scale (Fig. 1e)
mia scale
Silica layer Silica layer
Figure 2. TEM image of the interfacial area in sample 2 (Fig. 2a). details of the interface between the chromia scale and the ferrite (Fig. 2b). The silica layer is ~ 50 nm thick and does not form a continuous film.
417
Applying a classical 2 beam diffraction contrast method for measuring nanoprecipitate misfit L. Lae1, P. Donnadieu2 1. Société BASSETTI, 91bis avenue du Général Mangin, 38100 Grenoble France 2. SIMAP, INPGrenoble-CNRS-UJF, BP 75, 38402 Saint Martin d'Hères [email protected] Keywords: misfit, precipitate, 2-beam conventional TEM
Hardening precipitation remains of high interest for improving the mechanical properties of light alloys for structural applications. This precipitation occurs in the earliest stages of decomposition of a supersaturated matrix. The nanoscale precipitates which are often metastable are stabilized by elastic and interfacial energy. Hence particular attention is given to the misfit between the precipitates and the matrix. The precipitates being out of equilibrium, the misfit can be known only by direct measurement, basically by TEM because of the precipitate size (~ 5 to 20 nm). TEM provides numerous methods to measurement local deformation like CBED or HRTEM combined to the Geometric Phase Analysis. However because of the high particle density typical of hardening precipitation, CBED cannot be used as well as HRTEM when the precipitates are spherical. Ashby and Brown [1] have earlier established a method to measure the coherency strain for spherical precipitates using conventional TEM. Still the method has been rarely used quantitatively. As most of the CCD cameras are now able to record high contrast images, it seems interesting to revisit the possibility of the “Ashby and Brown” method. We have applied it to Al3(Sc,Zr) precipitates within the Aluminum matrix [2]. The composition of the precipitates is close to Al3Sc, though with a small amount of Zr . Figure 1a show the simulation of the BF image of a precipitate of radius r = 10 nm. The simulation is based on the Howie-Whelan equations under 2 beam conditions (g = (220)). The description of the displacement field is obtained using Eshelby description. Anomalous absorption and image forces were taken in account, the sample thickness is assumed to be 100 nm. As illustrated by Figure 1b, the simulated image intensity profile is very sensitive to the misfit value. Hence the Ashby and Brown method stands as a quite sensitive and appropriate method to measure the coherency misfit. Besides comparison of intensity profile can be simply used for determining the misfit. Figure 2 compares the experimental image and the experimental intensity profile to the one simulated for a misfit of 0.3 %. The method has been repeated on a limited number of precipitates. For precipitate with radius 9-10 nm, the misfit is 0.3 % while for larger precipitates (radius 14 nm), the misfit is 0.8 %. In any case the measured misfits are significantly smaller than 1.4 %, the value for bulk Al3Sc. The increase of misfit with the precipitate size is consistent with the high value for the equilibrium phase. However even the larger precipitates are far from the equilibrium value. Such difference points out the interest for direct
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 417–418, DOI: 10.1007/978-3-540-85226-1_209, © Springer-Verlag Berlin Heidelberg 2008
418
measurement on nanoprecipitates in view of a modelling taking in account the elastic energy. It should be emphasized that owing to the digitization facilities given by CCD cameras, the classical method of Ashby and Brown seems to be very relevant and quite simple to carry out for quantitative study of coherency strains of nanoparticles. 1. 2. 3.
M. F. Ashby and L. M. Brown Phil. Mag. 8 (1963) p.1083 A. Deschamps, L. Lae and P. Guyot, Acta Materialia, 55 (2007)p. 2775 Part of this work has been funded by the joint research program Precipitation between Pechiney, Usinor, CNRS, and CEA
b
a
Figure 1. Simulated Dark Field image of a coherent precipitate (radius 10 nm, misfit 0.2 %) (Fig. 1a) and the intensity profile of simulated images for misfit : 0.2 %, 0.5 % and 1% (Fig. 1b)
a
10 nm
b
Figure 2. Experimental BF image under 2 beam condition (Fig. 2a) Comparison of experimental and simulated intensity profile (misfit : 0.3 % ; precipitate size 9 nm, measured with DF images made on a superlattice spot).
419
Microstructure and interface composition of γ-phase in Co38Ni33Al29 shape memory alloy R. Espinoza1, B. Bartova1, D. Schryvers1, S. Ignacova2 and P. Sittner2 1. EMAT, University of Antwerp, Groenenborgerlaan 171, B-2020 Antwerp, Belgium 2. Institute of Physics ASCR v.v.i., Na Slovance 2, Prague 8, CZ-182 21, Czech Republic [email protected] Keywords: Shape memory alloys, interface, FIB
Ferromagnetic shape memory alloys (FSMAs) are being intensively studied because of their potential applications as smart materials. In these materials, the martensitic transformation processes can be triggered by applying a magnetic field, in addition to the conventional mechanism in SMAs. Recently, Co–Ni–Al alloys have attracted increasing interest as new FSMAs [1-4]. Due to their physical and mechanical properties they are also attractive as moderate high-temperature SMAs. The Co-Ni-Al system undergoes a martensitic transformation from β-phase (cubic ordered B2-type) austenite to L10 (tetragonal) martensite in a temperature range between -180 and 120°C [5]. However, the alloy is extremely hard and brittle in the polycrystalline state, and it was found that the presence of the secondary γ-phase significantly improves the poor ductility of Co–Ni–Al polycrystals [2, 4, 6]. Nevertheless, the exact role of the γ-phase in the martensitic behavior is not clear, e.g. by inducing nucleation points for the transformation, affecting composition, etc. On the other hand, the γ-phase is not homogeneously distributed at a small enough scale (Figure 1) [7], that easily allows the presence of an interface between phases in a regular TEM sample prepared by electropolishing. Because of this, an adequate study of the interface requires the use of an advanced preparation technique like Focused Ion Beam (FIB) to obtain samples for TEM. The objective of this work is to characterize the microstructure and composition of a Co38Ni33Al29 alloy in the interface between γ phase and the β- or martensite phases. After the identification of the γ-phase in a polished surface, the FIB technique allowed us to prepare samples at the desired position (Figure 2). The microstructure of the γphase was not affected during the sample preparation, showing a L12 ordered structure. The results obtained by EDX showed a local variation of the composition near the interface with the β-phase (Figure 3), which means a depletion of the Co content of around 6% (see Table I). 1. 2.
H.E. Karaca, I. Karaman, Y.I. Chumlyakov, D.C. Lagoudas, X. Zhang, Scripta Mater. 51 (2004), p. 261. R.F. Hamilton, H. Sehitoglu, C. Efstathiou, H.J. Maier, Y. Chumlyakov, X.Y. Zhang, Scripta Mater. 53 (2005), p. 131.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 419–420, DOI: 10.1007/978-3-540-85226-1_210, © Springer-Verlag Berlin Heidelberg 2008
420
3. 4. 5. 6. 7. 8.
Z.H. Liu, X.F. Dai, Z.Y. Zhu, H.N. Hu, J.L. Chen, G.D. Liu, G.H. Wu, J. Phys. D Appl. Phys. 37 (2004), p. 2643. R. Kainuma, M. Ise, C.-C. Jia, H. Ohtani, K. Ishida, Intermetallics 4 (1996) S151. K. Oikawa, L. Wulff, T. Iijima, F. Gejima, T. Ohmori, A. Fujita, K. Fukamishi, R. Kainuma, K. Ishida, Appl. Phys. Lett. 79(20) (2001), p. 3290. P.J. Brown, K. Ishida, R. Kainuma, T. Kanomata, K-U. Neumann, K. Oikawa, B. Ouladdiaf, K.R.A. Ziebeck, J. Phys. Condens. Mat. 17 (2005), p. 1301. B. Bartova, D. Schryvers, Z.Q. Yang, S. Ignacova, P. Sittner, Scripta Metall. 57(1) (2007), p. 37. Acknowledgements: R. Espinoza would like to thank to the Belgian Science Policy for the financial support. B. Bartova and S. Ignacova gratefully acknowledge financial support from the MULTIMAT Marie Curie Research Training Network (MRTNCT-2004-505226).
Figure 1. Microstructure of Co38Ni33Al29 alloy consisting of β-phase matrix with uniformly distributed γ-phase.
Figure 2. SEM image showing martensite and γ-phase at room temperature in the Co38Ni33Al29 alloy. Table I. Composition obtained by EDX of the points showed in Figure 3. Point 1 2 3 4 5 6 7
Figure 3. CoNiAl FIB TEM sample. The lighter zone in the middle (delimited by lines) corresponds to the γ-phase. The numerated points indicate the positions of EDX analysis.
Co 35.023 31.127 53.250 52.977 55.258 35.239 37.007
Ni 31.072 30.831 27.946 29.849 28.707 31.146 32.010
Al 33.682 37.326 18.239 16.868 15.683 33.465 30.454
421
Microstructural characterization of the aluminum alloy 6063 after work hardening treatments I.M. Espósito1,2, S.J. Buso1,2, W.A. Monteiro2,3 1. Centro Universitário Sant’Anna – São Paulo - Brazil 2. Instituto de Pesquisas Energéticas e Nucleares IPEN/USP– São Paulo - Brazil 3. Universidade Presbiteriana Mackenzie – São Paulo - Brazil [email protected] Keywords: Aluminum Alloys, Thermal Treatments, Electron Microscopy, Hardness
The aluminum 6063 alloy possesses a great industrial interest, presenting characteristics that justify its frequent use, when compared to the other aluminum alloys: the precipitation hardening and high cold work capacity. These alloys present high ductility, that allows their use in operations with high deformation degrees, as the cold work.[1,2] The aluminum alloys of the 6xxx series are used in a wide variety of applications, from the use in architecture profiles, as it is the case of the alloys more diluted and consequently of smaller mechanical resistance, as to 6063 and 6060, until the named alloys of structural application with larger tenors of alloying elements and higher hardness, with great application potential in the automotive industry, among other. [3] For this present work, samples of the commercial aluminum 6063 alloy bar (φ = 8 mm) was cold worked (90% area reduction) and then submitted to isothermal treatments at 735 K at 0, 60, 600 and 6000 s. Following the processes of analysis, samples for TEM were obtained, being the process of preparation the usual route. From the same lot a series of samples were prepared for hardness analysis. The observation of microstructure was made in a TEM JEOL JEM 200 C, available in CCTM of IPEN/USP and the hardness analysis in MICROMET Buehler from the Mechanical Engineering Department from USP, with a charge of 100 g. Figure 1 shows the evolution of microstructure of the alloy during the thermal treatments: 1a). a net of dislocations due to the high plastic deformation in sample without thermal treatment, 1b) a contour of grains showing a net of dislocations inside one of them due to the presence of precipitates Mg2Si for sample with 60 s of treatment, 1c) dislocations in an contour of grain, for sample with 6000 s of treatment. Figure 2 shows the hardness Vickers curve obtained for the samples in study. The analysis shows a decrease in hardness from 0 to 600 s of time of treatment, due to the recovery process in the final stage and simultaneously the recrystallization process. From the 600 s of treatment the hardness increases slightly due, mainly, to the presence of precipitates Mg2Si. 1. 2.
Espósio, I.M.; Buso, S.J.; Monteiro, W.A. Hardness analyses in an 6063 alloy after cold work and thermal treatments. In: International Materials Symposium, Materials 2005, Aveiro, Portugal, 2005. METALS HANDBOOK, ASM, 9th printing, v.14 Metals Park, Ohio, 1988, p.317-319
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 421–422, DOI: 10.1007/978-3-540-85226-1_211, © Springer-Verlag Berlin Heidelberg 2008
422 3.
Espósio, I.M.; Buso, S.J.; Monteiro, W.A. Análise da liga comercial 6063 após tratamentos termomecânicos. In: Congresso Brasileiro de Ciência e Engenharia de Materiais, CBCIMAT 2006, Foz do Iguaçu, Brazil, 2006.
(b)
(a)
(c)
Figure 1. TEM of samples of aluminum 6063 alloy 90% cold worked: 1a). a net of dislocations due to the high plastic deformation in sample without thermal treatment, 1b) a contour of grains showing a net of dislocations inside one of them due to the presence of precipitates Mg2Si for sample with 60 s of treatment, 1c) dislocations in an contour of grain, for sample with 6000 s of treatment.
Figure 2. Sequences of the analyses of DSC in samples of Al-2Mg-1Nb
423
Microstructure- mechanical property relationships in dual phase automotive strip steels V. Tzormpatzdi, and G. Fourlaris Laboratory of Physical Metallurgy, National Technical University of Athens, 9 Heroon Polytechniou St., 15780, Athens, Greece. [email protected] Keywords: dual phase, microstructure, mechanical properties, martensite
Dual phase (DP) and Transformation Induced Plasticity (TRIP) steels belong to the family of advanced high strength strip steels (AHSS) [1]. These steel grades are developed to permit the down-gauging of the body-in-white vehicle components, while providing high strength, suitable σ0 2% / tensile strength ratios, excellent formability and crash performance. The increased use of modern automobiles leads to the production of safe, fuel efficient and environmentally friendly vehicles. The objective of the present study is to assess the effect of variable intercritical annealing sequences to the microstructure and the attendant mechanical properties of two different dual phase strip steel grades. Intercritical annealing experiments were carried out for the DP800 and DP600 grades within the temperature range of 750 to 875oC, for time intervals ranging from 180 to 450s followed by water quenching. The microstructure was investigated using scanning electron microscopy (SEM) and X-ray diffraction. The mechanical properties were assessesd via Vickers hardness testing, while selective samples were tensile tested using standardized samples under static deformation conditions. The microstructure of the as received DP 800 steel is presented in Fig. 1, while that of the as received TRIP 600 is given in Fig.2. The experimental results showed that following intercritical annealing of the DP800 at 775oC for 180s the mechanical properties of the modified DP800 steel were enhanced (i.e. higher elongation values coupled with an improved σ 0 2%/tensile ratio of 0.48, while maintaining a UTS value of 800MPa-Fig.5). This has been attributed to the microstructural features of the modified DP800 product (Fig.3), i.e. refined martensite island dispersion at ferrite/ferrite grain boundaries, while maintaining a martensite volume fraction of 39%. Similar attempts of enhancing the mechanical properties of DP600 were met with less success, since a significant increase of the tensile strength of intercritically annealed DP600 samples was measured, for the intercritical annealing temperatures and cooling regimes employed (Fig. 4). The present study has demonstrated that under carefully controlled processing conditions it is entirely feasible to obtain modified microstructures in DP800 grades with a desirable mix in terms of the martensite to ferrite ratio, and with suitable martensite particle dispersions characteristics, leading to the production of enhanced DP800 strip steel products. Such a goal has not been accomplished, as yet, for the DP600 grade.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 423–424, DOI: 10.1007/978-3-540-85226-1_212, © Springer-Verlag Berlin Heidelberg 2008
424 1. 2.
1. Senuma T. ISIJ International, 41 (2001) 520-532 2. Rocha R.O., Melo T.M.F., Pereloma E.V.,Santos D.B.Mat. Sci. and Eng.A, 391(2005) 296-304
Figure 1. SEM micrograph of DP800 strip steel in the as received condition
Figure 2. SEM micrograph of DP600 strip steel in the as received condition
Figure 3. DP800 intercritically annealed at Figure 4. DP600 intercritically annealed at 775oC for 180sec, water quenched 775oC for 180sec, water quenched
Figure 5. Curve presenting the σ 0 2% / UTS versus UTS
425
Electron diffraction analysis of nanocrystalline Fe-Al C. Gammer, C. Mangler, C. Rentenberger and H.P. Karnthaler Physics of Nanostructured Materials, Faculty of Physics, University of Vienna, Boltzmanngasse 5, 1090 Vienna, Austria [email protected] Keywords: Electron diffraction, peak broadening, nanocrystalline materials
Finite grain sizes lead to a broadening of diffraction peaks. For defect free grains the median grain size (Dmed) can be determined from the half width at half height (∆g) of a diffraction peak using the Scherrer equation (Dmed=0.443·(∆g)-1) [1]. In the present work this equation is applied for using TEM methods to determine the size of grains, the size of coherently scattering domains (CSD) and that of ordered domains. Disordered nanocrystalline Fe-45at.%Al was produced by high pressure torsion (HPT) from B2 ordered material [2]. Samples annealed to different temperatures were investigated. Their diffraction profiles were deduced by ring integration of the TEM diffraction images and the peak broadening was determined by fitting Voigt peakfunctions. Images were taken using a TEM operating at 200kV. The instrumental peak broadening can be deduced from the width of diffraction spots of a single crystal. To compensate for this, the results were deconvoluted. Figure 1 shows a bright-field image and the diffraction pattern of a sample that is disordered and nanocrystalline after HPT; the grain boundaries are not well defined. Annealing the sample to 370°C (cf. Fig. 2) leads to defect recovery and to the restoration of the B2 structure. The latter correlates with the appearance of the (100) superlattice reflection (cf. Fig. 2b). From the width of the different reflections in the diffraction profiles (cf. Fig. 3) median domain sizes were calculated (cf. Fig. 4). The deduced values using fundamental reflections (110) and (200) reflect the CSD because of the high density of defects within the grains. With increasing annealing temperature the CSD size increases. Using TEM dark-field images (with fundamental reflections) the grain size at 370°C was found to be log-normal distributed with a median of 38±4 nm, that is higher than the CSD size as not all the defects are recovered. The ordered domain size estimated from the (100) peak width approaches the CSD size and is in good accordance with results from TEM dark-field images using a (100) reflection. From the present results it can be concluded that in nanocrystalline materials the Scherrer equation is a very powerful tool for using TEM methods to estimate median grain and domain sizes using both fundamental and superlattice reflections. 1. 2. 3.
F. Fultz and J.M. Howe, “Transmission Electron Microscopy and Diffractometry of Materials” (Springer Verlag, Berlin Heidelberg) (2008), p.425 C. Mangler, C. Rentenberger, I. Humer, L. Reichhart and H.P. Karnthaler, Microscopy and Microanalysis 13 (2007), p.298 We acknowledge support by the research project “Bulk Nanostructured Materials” of the research focus “Materials Science” of the University of Vienna and by the Austrian research fund FWF.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 425–426, DOI: 10.1007/978-3-540-85226-1_213, © Springer-Verlag Berlin Heidelberg 2008
426
Figure 1. Fe-45at.%Al deformed by HPT with a shear strain of 10 000%. (a) TEM bright-field image. (b) corresponding diffraction pattern.
Figure 2. Fe-45at.%Al deformed by HPT (10 000%) and annealed at 370°C. (a) TEM bright-field image. (b) corresponding diffraction pattern.
Figure 3. Diffraction profile of Fe45at.%Al deformed by HPT (10 000%) and annealed at 170°C. Superlattice reflections are indicated in bold.
Figure 4. Variation of the median coherently scattering domain sizes compared to the ordered domain sizes.
427
Dual Beam and TEM characterisation of deformation structures in fatigued austenitic stainless steel A. Garcia1,2, L. Legras1, M. Akamatsu1 and Y. Bréchet2 1. EDF R&D, Les Renardières, Département MMC, 77818 Moret sur Loing, France 2. SIMAP, INPGrenoble, CNRS UJF, Domaine Universitaire, BP 75, 38402 Saint Martin d’Hères cedex, France anais.garcia@edf fr Keywords: austenitic stainless steel, fatigue, dislocations structures, TEM, Dual Beam.
Thermal fatigue cracking is a damaging mode of austenitic stainless steels, particularly in the mixing zone of the Residual Heat Removal system (RHR system) of Pressure Water Reactor (PWR). The aim of this research project is to study and compare the deformation microstructures, at crack-tips and in the bulk, observed on a pulled out structural component made of AISI 304L stainless steel and those developed during cyclic deformation, on low cycle fatigue standard specimens. Such a comparison of the deformation microstructures could give key indicators of the real magnitude of the mechanical solicitation undergone by the pulled out structural component. First, this study is devoted to identify the microstructures developed in the bulk of fatigued AISI 304L specimens. For this purpose, total-axial-strain-controlled low cycle fatigue tests, performed in air and PWR water, at 150°C and 300°C, with 0,10% and 0,50% total strain amplitudes, are used. The microstructural characterization is carried out by Transmission Electron Microscopy (TEM), on a FEI Tecnai G2 F20 operating at 200kV. At the lowest strain amplitude, for each temperatures and environments, planar dislocation arrays and stacking faults on {111} easy glide planes prevail. Whereas, at the highest strain amplitude, the superposition of planar slip on {111} planes with the ladder-like or wall and channel structure of persistent slip bands (PSB), presented in Figure 1a, and cells predominate. Among the three variable parameters of the fatigue tests, the strain amplitude is the most influent one on the observed deformation microstructure. These structures are known to be characteristic of austenitic stainless steel with intermediate stacking fault energy (SFE) [1-4]. Misorientation between cells is also measured in TEM, thanks to the ACT facility developed by Dingley and Wright [5], which uses reconstructed diffraction patterns from conical dark fields. Besides, deformation microtwins, presented in Figure 1b, are detected in PWR water at 300°C for both strain amplitudes. The twinning plane is the (111) plane which is determined by a combined analysis of the SAD pattern [6] with the transformation matrix for deformation twinning calculated by Mahajan [7]. Second, the RHR system’s microstructure is compared to the results previously presented in this paper. Planar dislocation arrangements and microtwins along {111} planes are observed in the pulled out specimen, which is similar to the microstructures detected in standard fatigued specimen cycled at low strain amplitude and high temperature.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 427–428, DOI: 10.1007/978-3-540-85226-1_214, © Springer-Verlag Berlin Heidelberg 2008
428
Last, the microstructures observed along cracks of the RHR component are analysed by TEM, using cross section samples prepared using GATAN PIPS, and by an FEI Helios Nanolab Dual Beam, equipped with an HKL Nordlys CCD camera and with 3D imaging and EBSD softwares (AutoSliceAndView and AutoReveal). It allows to prepare thin foils in very precise zones along the crack, at its vicinity and at the cracktip. Cross section samples, localised on the structural component’s crack, points out the presence of oxide at the crack-tip and of nano-steps on the crack edges. Moreover, the low dislocation density observed at the crack tip indicates that the residual plastic stresses and the plastic deformation are rather low in this area. Works are carried out by Dual Beam in order to build a 3D representation of the dislocations structures, from series of Electron Channeling Contrast Images (ECCI), using the Forescatter detector (FSD) located at the bottom of the EBSD detector. 1 2. 3. 4. 5. 6. 7.
F. Ackermann, L.P. Kubin, J. Lepinoux, and H. Mughrabi, Acta Metall. 32 (1984), p. 715. M. Gerland, J. Mendez, P. Violan and B. Ait Saadi, Mater. Sci. Eng. A118 (1989), p. 83. C. Laird, Z. Wang, B.T. Ma and H.F. Chai, Mater. Sci. Eng. A113 (1989), p. 245. K. Obrtlík, T. Kruml and J. Polák, Mater. Sci. Eng. A187 (1994), p. 1. S.I. Wright and D.J. Dingley, Materials Science Forum 273-275 (1998), p. 209. T.H. Lee, C.S. Oh, S.J. Kim and S. Takaki, Acta Mater. 55 (2007), p. 3649. S. Mahajan, Metallography 4 (1971), p. 43.
Figure 1. TEM micrographs of AISI 304L steel cycled with Δεt/2 = 0,50 % (a) coexistence of cells, PSB and planar slip (b) microtwins in PWR water at 300°C. 80 70
Ni Fe Cr
60
g = [ 1 10]
50 40 30 20 0 0 0
0
20
30
40
50
100 nm
Figure 2. TEM micrographs of a secondary crack in the RHR system (a) propagation with nano-steps (b) Presence of oxide at the crack-tip revealed by an EDX profile.
429
Microstructural characterisation of steel heat-treated by the novel quenching and partitioning process K. He1, D.V. Edmonds1, J.G. Speer2, D.K. Matlock2 and F.C. Rizzo3 1. Institute for Materials Research, School of Process, Environmental and Materials Engineering, University of Leeds, Leeds LS2 9JT, United Kingdom 2. Advanced Steel Processing and Products Research Centre, Colorado School of Mines, Golden, CO 80401, USA 3. Department of Materials Science and Metallurgy, Pontifícia Universidade CatólicaRio de Janeiro; RJ 22453-900, Brazil k [email protected] Keywords: steel, quenching and partitioning, microstructure
The Quenching and Partitioning (Q&P) process, a new development in steel heat treatment, is designed to create mixed martensite/retained austenite steel microstructures [1,2]. It involves partial transformation of austenite to martensite by interrupted quenching to a temperature (QT) between the martensite start and finish temperatures, followed by annealing at a partitioning temperature (PT) designed to enrich the remaining austenite with carbon, thereby stabilizing it against further transformation to martensite upon subsequent cooling to room temperature. Cementite precipitation in martensite is suppressed by alloying with Si or Al, thereby increasing the time for carbon to escape supersaturation by diffusion into adjacent untransformed austenite. This philosophy is similar to that used to produce carbide-free bainitic structures [3], of current interest in the development of TRIP-assisted automotive sheet steels [4]. Potential advantages of Q&P are: high strength from martensite fraction; exceptionally high carbon concentration of austenite fraction, which is decoupled from austenite decomposition as compared with carbon partitioning during the bainite transformation; fast processing limited only by the rapid diffusion of carbon. Microstructural evolution during Q&P processing of medium-carbon austenite (steel composition: 0.6C-0.95Mn-1.96Si-wt%) for various quenching and partitioning temperatures and partitioning times was examined using light optical and transmission electron microscopy. Comparison was made between the microstructural characteristics of fully austenitised Q&P treated samples and ones subjected to bainitic treatments. Figures 1 and 2 illustrate microstructures after Q&P treatment compared with conventional bainitic treatment. Both Q&P samples, partitioned at 400 and 500°C, possess uniform fine microstructure after short annealing times (Figs 1a and 1b). However, characteristically, the bainite transformation was incomplete at 400°C after shorter annealing times, only partially decomposing the austenite (Fig 1c), and required a much longer time to develop similarly uniform microstructures of carbide-free bainite (Fig 1d). Examination by TEM similarly reveals a finer, more uniform Q&P structure of martensite laths interwoven with retained austenite (Fig 2a and b) produced at the
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 429–430, DOI: 10.1007/978-3-540-85226-1_215, © Springer-Verlag Berlin Heidelberg 2008
430
shorter annealing times compared with the bainite structure of bainitic ferrite interwoven with retained austenite (Fig 2c) achieved in the same steel composition. These results indicate that Q&P processing can produce refined homogeneous microstructures with substantial fractions of stabilized retained austenite, and generally within a time scale likely to be much shorter than that of a conventional bainite treatment, which may be of importance to industrial steel heat treatment procedures. 1. 2. 3. 4.
J.G. Speer et al., Acta Mater. 51 (2003), p. 2611. D.V. Edmonds et al., Mater. Sci. Eng. A438-440 (2006), p. 25. H. K. D. H. Bhadeshia and D. V. Edmonds, Metall. Trans. 10A (1979), p. 895. D. K. Matlock and J. G. Speer, in “Proc. 3rd Int. Conf. Structural Steels”, ed. H.C. Lee, (The Korean Institute of Metals and Materials, Seoul, Korea) (2006), p. 774.
(a)
(c)
(b)
(d)
(a)
(b)
(c)
Figure1. Light optical micrographs: (a) QT=190ºC and PT=500ºC for 10s; (b) QT=190ºC and PT=400ºC for 120s; (c) bainitic treatment 400ºC for 120s; (d) bainitic treatment 400ºC for 900s.
Figure2. TEM micrographs: (a) QT=190ºC and PT=500ºC for 10s (bright-field and centred dark-field image using (220)γ); (b) QT=190ºC and PT=400ºC for 120s (centred dark-field image using (002)γ); (c) bainitic treatment 400ºC for 120s.
431
Martensite tempering behaviour relevant to the quenching and partitioning process K. He1, D.V. Edmonds1, J.G. Speer2, D.K. Matlock2 and F.C. Rizzo3 1. Institute for Materials Research, School of Process, Environmental and Materials Engineering, University of Leeds, Leeds LS2 9JT, United Kingdom 2. Advanced Steel Processing and Products Research Centre, Colorado School of Mines, Golden, CO 80401, USA 3. Department of Materials Science and Metallurgy, Pontifícia Universidade CatólicaRio de Janeiro; RJ 22453-900, Brazil k [email protected] Keywords: steel, tempering, carbide
The Quenching and Partitioning (Q&P) process is a steel heat treatment to create microstructures with retained austenite [1,2]. It involves quenching austenite to between the martensite start and finish temperatures, followed by a partitioning treatment to enrich the untransformed austenite with carbon, thereby stabilizing it to room temperature. Carbon partitioning to austenite, however, is competitive with carbide precipitation [2] and so Si and/or Al alloying is suggested and employed in order to suppress cementite formation to protect carbon. However, previous studies show that alloying is ineffective against transitional epsilon carbide precipitation [2]. Consequently, it is important to understand the effects of Si and Al on tempering behaviour relevant to a Q&P treatment of steel. Microanalytical electron microscopy has thus been used to determine the compositions of epsilon carbide and cementite and the epsilon to cementite transition during tempering of quenched Si- and Al-containing high-purity Fe-C alloys. In Fe-0.6C-1.97Si, tempered in the range 200-500°C, transitional epsilon carbide and equilibrium cementite were both observed (Figure 1), but within different time frames, as indicated by the schematic transition line in Figure 2. Epsilon carbide forms first but is succeeded by cementite after increasing times at decreasing temperatures, e.g. 5, 10 and 70 min at 500ºC, 450ºC and 400ºC, respectively. STEM-EDX analysis of epsilon carbides and adjacent ferrite using a 1nm probe showed no composition difference between them i.e. the transitional carbide possessed a Si concentration similar to that of the surrounding matrix. In contrast, TEM-EDX analysis of cementite precipitates detected negligible Si. These recent analyses are confirmation of early reported studies [3-5] and reinforce the generally accepted argument that Si influences the formation of cementite because its low solubility requires rejection during carbide formation [3]. Knowledge of the temperature-time transition line would be useful for optimizing the partitioning condition for Q&P treatment of steel. For the two partitioning conditions indicated in Figure 2, even though both lie within the epsilon carbide region, T1t1 is favoured over T2t2, because at higher tempering temperature the driving force for epsilon carbide formation is reduced and this condition is closer to the transition from S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 431–432, DOI: 10.1007/978-3-540-85226-1_216, © Springer-Verlag Berlin Heidelberg 2008
432
epsilon to the more stable cementite phase. In addition, epsilon carbide formation must compete with the escape of carbon from martensite to austenite in a Q&P treated microstructure, calculated to be extremely rapid [6] (especially at higher temperatures, although probably hindered by trapping at sites within the martensite). With decreasing carbon supersaturation, the driving force for carbide precipitation is also further reduced. In Fe-0.6C-2.41Al, TEM observations showed that Al addition gave similar results to Si in terms of carbide composition and precipitation behaviour. As for Si alloying, Al did not suppress formation of epsilon carbide. At 450ºC the epsilon carbide to cementite transition was observed at around 10min, similar to that for Si alloying. (a)
(101)ε+(101)
(b)
(010)ε
(c)
(d)
(-11-1)ε
Figure 1. Fe-0.6C-1.97Si: (a) STEM bright-field image of epsilon carbides, 300°C for 15min; (b) bright-field and centred dark-field images using (-1,1,-1)ε reflection, 410°C for 15min; (c) corresponding electron diffraction pattern; (d) centred dark-field image using (312) cementite reflection, 460°C for 15min.
Figure 2. Schematic TemperatureTime diagram of the epsilon carbide to cementite transition.
1. 2. 3. 4. 5. 6. 7.
J.G. Speer et al., Acta Mater. 51 (2003), p. 2611. D.V. Edmonds et al., Mater. Sci. Eng. A438-440 (2006), p. 25. W.S. Owen, Trans ASM 46 (1954), p. 812. J. Gordine and I. Codd, J. Iron Steel Inst. 207 (1969), p. 461. W. C. Leslie and G.C. Rauch, Metall. Trans. 9A (1978), p. 343. F.C. Rizzo et al., in “Solid-Solid Phase Transformations in Inorganic Materials”, ed. J.M. Howe et al., (TMS, The Minerals, Metals & Materials Society, Warrendale, PA, USA) (2005), p. 535. Acknowledgement to the UK North-West Fine-Probe Microanalytical STEM Facility.
433
Chemical and structural analysis of NiAl-Al2O3 interface by FETEM and STEM W. Hu1, T. Weirich2 and G. Gottstein1 1. Institut of Physical Metallurgy and Metal Physics, RWTH Aachen University 2. Central Facility for Electron Microscopy, RWTH Aachen University [email protected] Keywords: interface structure, chemistry, FETEM, STEM
In continuous ceramic fiber reinforced intermetallic matrix composites (IMC) the interfacial shear strength plays an essential role for the load transfer from the matrix to the fiber and determines the strength and ductility of the IMCs. The interfacial strength is controlled by the interface structure and chemistry which developed during the IMCfabrication process. The present investigation focused on the evolution of interface structure and chemistry of NiAl coated Sapphire-fibers during composite fabrication (fiber coating, diffusion bonding and embedded casting). The interface structure of the as-coated fiber is shown by a bright field EFTEM micrograph in Figure 1a. It reveals a layer of several 10nm thickness between fiber and NiAl. HRTEM images demonstrate that this interface layer has an amorphous structure (see Figures 1b and c) and consisted of oxygen, aluminium and nickel, as shown in the element mapping taken by EFTEM (Figures 1d-f). The composition of the layer was semi-quantitatively analysed with STEM/EDX. It contained about 60 at.% oxygen, 20~30 at.% Al and 10~20 at.% Ni. Thus, this amorphous interface layer was identified as a compound (Al,Ni)-oxide. This amorphous interface formed by incorporation of Al and Ni with the remaining moisture of the residual gas in the reaction chamber during the vapor phase growth in high vacuum during the initial stage of the PVD-process, and caused a reactive thin amorphous oxide film on the fiber surface. After diffusion bonding (1300 °C/40 MPa/1h) the amorphous interface layer still existed between fiber and matrix (Figure 2a), but many nanocrystalline particles precipitated either in the amorphous layer or at the boundary between the layer and NiAl as well as the fiber (Figure 2b). Element maps obtained by EFTEM reveal several regions in the layer with enrichment of Al or Ni. The regions with high Al concentration corresponded to those of high oxygen content (Figures 2d and e). The areas of high Niconcentration are well separated from those of high O/Al-concentration (Figure 2c). We assume that these Al/O- or Ni-enriched areas correspond to those with nanocrystalline precipitates which were observed by HRTEM (Figure 2b). Furthermore, there existed also a thin continuous sublayer with a thickness of about 2~3 nm between the NiAl and the interface layer that contains large amounts of Al and oxygen (Figures 2d and e) and thus, was identified as Al-oxide. The interface structure and chemistry of NiAl-composites after casting at about 1700 °C are shown in Figure 3. There is still a continuous layer at the interface, merely the layer has a thickness of about 2~3 nm (Figure 3a). HRTEM reveals that this thin layer
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 433–434, DOI: 10.1007/978-3-540-85226-1_217, © Springer-Verlag Berlin Heidelberg 2008
434
consists of two different sublayers. An element line profile across the interface from positions A to D, taken by a STEM/EDXS-analysis suggests that the interface thin layer is composed of two sublayers: one is the Ni-rich sublayer at position C (thickness<2 nm) adjacent to the NiAl-matrix. This sublayer is likely a nickel-rich nickel aluminide with a Ni/Al-ratio ≈ 1.17. The other sublayer consists of Al-oxide and is located at position B (thickness<2 nm) in vicinity of the Al2O3-fiber (Figure 3b). These two sublayers of nickel aluminide and Al-oxide shown in the element line profile apparently correspond to the ones displayed in Figure 3a. Formation of an Al-oxide sublayer at the boundary with NiAl (Figure 2) and with nickel-rich nickel aluminide (Figure 3) led to a NiAl/Al2O3-bonding that caused a high interfacial shears strength due to a large work of adhesion between Al NiAl -O and NiAlAl 2 O 3 and consequently a high strength of NiAl composites. a
c
Al K-edge
e
NiAl NiAl
Al 2 O 3
Amorph. layer
b
2 nm Ni L 23-edge
d
O K-edge
f
Amorph. layer
Al 2O 3
2 nm
N i L 2 3 -e d g e
c
a a
O K -e d g e
e
Figure 2. Interface structure of asdiffusion bonded NiAl composite (a) bright field EFTEM image shows the interface structure, (b) HRTEM image shows the fine structure of the interface layer. (ce) element mapping in the area of Figure 2a, (f) results of semiquantitative STEM/EDX-analysis at the locations A-E in Figure 2a.
A l2O 3 A B N iA l C
E D
50 nm
b
A l K -e d g e
d
d = 0 25 24
Ni
In te rfa c e la ye r
.2 =0
09
Ni-rich sublayer
Al-rich sublayer Al2O3
Al
O
A
5 0 .7
4 4 .9
4 .3
B
0 .0
3 9 .9
6 0 .1
C
m 8n
1 1 .6
4 4 .1
D
100
0 .0
0 .0
E
7 1 .9
2 8 .1
0 .0
4 4 .3
b
NiAl
Figure 3. Interface structure and chemistry of an as-cast composite. (a) a bright field EFTEM image reveals the interface structure, (b) element profile across the interface along the white line in Fig. 3a.
Ni
600
400
Al
Counts
a
f S T E M /E D X -a n a lys is (a t.% ):
nm
d
A
B C
200
D
O 0
3 nm
Figure 1. Interface structure and chemistry of as-coated fiber. (a) bright field EFTEM image shows the interface structure, (b-c) HRTEM image reveals the fine structure of the interface, (d-f) EFTEM element mapping in the interface area shown in Figure 1a.
0
5
10 Postion (nm)
15
20
435
TEM investigations of aluminum precipitate in eutectic Si of A356 based alloys Z.H. Jia1, L. Arnberg1, P. Åsholt2, B. Barlas3, T. Iveland2 1. Department of Materials Science and Engineering, Norwegian University of Science and Technology, Alfred Getz vei 2b, N-7491 Trondheim, Norway 2. Hydro Aluminium R&D Sunndal, N-6601 Sunndalsøra, Norway 3. Montupet SA, 60181 Nogent sur Oise Cedex, France Zhihong.jia@material ntnu.no Keywords: precipitate; aluminum alloy; electron microscopy
Solidification of hypoeutectic type A356 alloys start with growth of primary aluminum (α-phase), followed by Al-Si eutectic [1]. Precipitation of Si, together with other added elements from aluminum has been extensively studied [2, 3]. However, little detailed characterization has been done on the eutectic Si phase. Recently, nanoscale precipitates have been observed in the Si phase [4, 5] and have been confirmed to be aluminum [6], which exhibit three preferential orientation relations with the Si matrix [001]Si║[111]Al; [111]Si║[001]Al; (110)Si║(1-10)Al. The present work gives more information about such aluminum precipitates based on electron microscopy. A356 based alloys were cast in a steel chill mould. Both as-cast and solution-treated samples were studied by (scanning) transmission electron microscopy (STEM). Thin foils were prepared by ion polishing with high purity Ar+ at 4 keV. A JEOL-2010F microscope equipped with an energy dispersive x-ray spectroscopic (EDXS) detector was used. Linescan analysis in STEM mode was performed with a probe of 0.7 nm. Aluminum precipitates with diameters in a range of 10-25 nm were observed in both as-cast and subsequently heat treated samples (Figure 1) and their morphology and size were found to be insensitive to heat treatments. Additional alloying elements did not affect the precipitate composition. The shape of precipitate rich areas varied from one eutectic Si particle to another, but most of them showed a sharp boundary which separated precipitate rich areas from precipitate free areas. Bright field STEM image revealed precipitates including dark “head”. HRTEM images (Figure 2) and linescan analysis of selected precipitate showed that such dark “head” to be composed of Si. Oxygen impurities are postulated to gather aluminum and stabilize aluminum precipitates [5]. However, the present EDS analyses did not show higher level of oxygen from precipitates as compared to the Si matrix. It is suggested, based on the present results, that the formation of aluminum precipitates is probably related to the observed dark “head” [7]. 1. 2. 3. 4. 5.
L. Lu, K. Nogita, S. D. McDonald, A. K. Dahle, JOM 56 (2004) 52. H. Y. Kim, T. Y. Park, S. W. Han, H. M. Lee, J. Cryst. Growth 291 (2006) 207. Q. G. Wang, C. J. Davidson, J. Mater. Sci. 36 (2001) 739. S. C. Hogg, C. J. D. Hetherington, H. V. Atkinson, Phil. Mag. Lett. 80 (2000) 477. D. K. Sadana, M. H. Norcott, R. G. Wilson, U. Dahmen, Appl. Phys. Lett. 49 (1986) 1169.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 435–436, DOI: 10.1007/978-3-540-85226-1_218, © Springer-Verlag Berlin Heidelberg 2008
436
6. 7.
W. T. Donlon, Metall. Mater. Trans. 34A (2003) 523. The work has been conducted within the FONDAL project which is a cooperation NTNU, CNRS, Hydro Aluminium and Montupet SA. The authors would like to acknowledge financial support from the French-Norwegian Foundation for Scientific and Technical and Industrial Research as well as from Hydro Aluminium and Montupet SA.
Figure 1. (a) bright field TEM image showing a eutectic Si particle in A356 based alloy. Small precipitates are observed in a part region of Si particle. There is an obvious boundary separating precipitate area from unprecipitate area (marked by arrow). (b) intermediate magnification image from an area of (a) showing highly dense precipitates of 10-25 nm in diameter. (c) Bright field STEM image showing spheroidal morphology of precipitate including a dark “head”.
Figure 2. High resolution TEM images of precipitates taken along different zone diffractions (a) Si [111] and (b) Si [-4-8-9]. Moiré fringes are caused by different lattice constants of Al and Si structure. The dark “head” shows the same lattice fringe as the Si matrix. There is a detectable interface between Al-precipitate and its dark “head”.
437
Microstructure of slow-cooled wedge-cast Cu58Co42 alloy with a metastable liquid miscibility gap E. Johnson1,2, S. Curiotto2, N. Pryds3 and L. Battezzati4 1. Niels Bohr Institute, Nano Science Center, University of Copenhagen, Denmark 2. Materials Research Department, RISØ DTU, Roskilde, Denmark 3. Fuel Cell and Solid State Chemistry Department, RISØ DTU, Roskilde, Denmark 4. Dipartimento di Chimica, IFM, Centro di Eccellenza NIS, University of Torino, Italy Erik Johnson, johnsonfys ku.dk Keywords: Cu-Co alloys, Liquid immiscibility gap, Microstructure
The Cu-Co equilibrium phase diagram (figure 1) contains a metastable liquid phase miscibility gap where the liquid phase will separate into two, provided it can be undercooled sufficiently before solidification sets in [1]. This has been achieved by casting a Cu58Co42 alloy in a wedge-shaped mould where the as-cast microstructure showed evidence for liquid phase separation prior to solidification, e.g. formation of Co-rich droplets in a Cu- rich matrix [2,3]. Using backscattering SEM the dark Co-rich phase can easily be distinguished from the bright Cu-rich matrix (figure 2). The big dark particles are the Co-rich droplets that solidified after phase separation in the undercooled liquid. As cooling progressed in the liquid droplets the composition of the Co-rich phase would change and small droplets of Cu-rich liquid would form and be pushed towards the interior leaving the rim unaffected. TEM samples of the wedge-cast material proved to be difficult to produce by electropolishing due to the coarseness of the microstructure, and ion milling was found to be the only preparation technique that gave reasonable result albeit both phases were saturated with radiation damage in form of dislocation loops and tangles. Figure 3 shows low magnification bright-field TEM images from two different samples. The shape of the Co-rich particles is mostly spherical in accordance with their initial formation as liquid droplets. The larger Co-rich particles (figure 3a) can be recognized from the radiation damage structure that is denser than in the Cu-rich matrix which often contains a high density of semi coherent Co precipitates formed in secondary solid state reactions. The size of the smallest Co-rich particles appears to be as small as 50100 nm (figure 3b) while it is difficult to ascertain smaller particles due to the radiation damage induced dislocation loops. X-ray diffraction showed that both phases have fcc structure and that the lattice parameters deviated with less than 1%. This means that the two phases – Co-rich droplets and Cu-rich matrix - often are aligned and essential grow as larger single crystals. The interface boundaries are hence pure chemical interfaces with structural integrity across the boundaries. The small mismatch between the two phases is reflected in the misfit dislocation distributions in the interfaces (figure 3) that can easily be confused with moiré fringes (figure 2a).
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 437–438, DOI: 10.1007/978-3-540-85226-1_219, © Springer-Verlag Berlin Heidelberg 2008
438 1. 2. 3. 4.
Y. Nakagawa: Acta Metallurgica, 6 (1958), p. 704. S. Curiotti, N. Pryds, E. Johnson, L. Battezzati, Mater. Sci. Eng. A, 449-451 (2007), p. 644. S. Curiotto, N. Pryds, E. Johnson, L. Battezzati, Met. Mater. Trans. A, 37A (2006), p. 2361. The work has been supported by the European Space Agency within the project “CoolCop” (ESA-MAP AO 99-010) and by the Danish Natural Science Research Councel.
1800 1700
s ta b le p h a s e d ia g ra m m is c ib ility g a p
γ
L iq u id
T [K]
1 6 0 0 C o -ric h 1500 1400 1300 1200 0 ,0
γ
C u -ric h
0 ,2
0 ,4 0 ,6 x (C u )
0 ,8
1 ,0
Figure 1. Cu-Co equilibrium phase diagram showing the occurrence of the metastable liquid miscibility gap. The arrow indicates the alloy composition.
Figure 2. SEM backscattering image from slow-cooled wedge-cast Cu58Co42 sample showing liquid phase separation that has led to formation of Co-rich droplets and particles dispersed in the Cu-rich matrix.
Cu-rich
1 μm
500 nm
Figures 3a and b. TEM of Co-rich particles formed by phase separation in the undercooled liquid in a Cu58Co42 slow-cooled wedge-cast sample. Most Co-rich particles have spherical shape.
100 nm
Co-rich
Figure 4. Interphase between a Co-rich particle and the Cu- rich matrix. The boundary separates phases with different composition but similar crystallography.
439
TEM investigations of Elektron 21 magnesium alloy after long-term annealing A. Kielbus Silesian University of Technology, Katowice, Poland andrzej [email protected] Keywords: Elektron 21, magnesium alloy, long-term annealing, TEM, microstructure
The paper presents results of TEM investigations of Elektron 21 magnesium alloy in as cast condition and after long-term annealing. Elektron 21 is magnesium based casting alloy containing rare earth (Nd and Gd) for used to at 200°C in aerospace application. It has high strength, good corrosion resistance and excellent castability [1]. Magnesium alloys containing neodymium and gadolinium are characterised by high-strength and good creep-resistant alloys for automotive and aerospace applications [2,3]. The rare earth elements have beneficial effect of on the creep properties and thermal stability of structure and mechanical properties of magnesium alloys [4]. The strength of magnesium alloys with RE is achieved essentially via precipitation strengthening. These alloys precipitate from the solid solution according to the sequence of phases: αMg→β”→β’ →β [5]. The material for the research was a casting Elektron 21 magnesium alloy. The chemical composition of this alloy is provided in Table 1. Solution heat treatment was performed at 520°C/8 h/water. Ageing treatment was performed at 200°C/16h/air. Long-term annealing was performed at 350°C/100÷2000h and then quenched in air. The microstructure of Elektron 21 alloy was examined by a Philips CM 20 Transmission Electron Microscope. The microstructure of Elektron 21 consists of primary solid solution α grains with eutectic α + Mg12(Ndx,Gd1-x) phase at grain boundaries (Fig.1). The Mg12(Ndx,Gd1-x) phase is a modification of Mg12Nd phase with neodymium substituted by gadolinium due to reasonably small difference in the atomic radii. After solution treatment the Mg12(Ndx,Gd1-x) phase dissolved in the matrix. Aging at 200°C/16h leads to precipitation of β’ phase (Fig.2). After annealing at 350°C/100h the microstructure consists of β phase precipitates inside solid solution grains (Fig.3) and singular precipitates of Mg41Nd5 phase on grain boundaries. With continued ageing at 350°C (5000h) the volume fraction of Mg41Nd5 increase. The precipitates of this phase create the characteristic network on grain boundaries. Also the regular precipitates of Mg3Gd phase have been observed (Fig.4) 1. 2. 3. 4. 5.
P. Lyon, T. Wilks, I. Syed, Magnesium Technology (2005), p.303. H. Friedrich, S. Schumann, Journal of Materials Processing Technology, Vol. 117, Issue 3 (2001), p. 276. B. Mordike, Materials Science and Engineering, A324 (2002), p.103. B. Mordike, Journal of Materials Processing Technology, Vol. 117, Issue 3 (2001), p.391. B. Smola, I. Stulikova, F. von Buch, B. Mordike, Materials Science and Engineering A, 324, Issue 1-2 (2002), p.113.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 439–440, DOI: 10.1007/978-3-540-85226-1_220, © Springer-Verlag Berlin Heidelberg 2008
440
6.
The present work was supported by the Polish Ministry of Science and Higher Education under the research project No N N507 451334 “Structural stability of Mg-RE-Zr magnesium alloys in simulated working conditions”.
Table I. Chemical composition of the Elektron 21 magnesium alloy in wt.-%. Gd Nd Zr Zn Mn Fe Ag Mg 1,2 2,7 0,49 0,4 0,001 0,003 0,01 balance
Figure 1. Eutectic α + Mg12(Ndx,Gd1-x) in Elektron 21 alloy in as-cast condition.
Figure 2. β’ precipitates in Elektron 21 alloy after aging at 200°C/16h.
Figure 3. β precipitates in Elektron 21 alloy after annealing at 350°C/100h.
Figure 4. Mg41Nd5 and Mg3Gd precipitates in Elektron 21 alloy after annealing at 350°C/2000h.
441
Microstructure of AJ62 magnesium alloy after long-term annealing A. Kielbus1 and J. Mizera2 1. Silesian University of Technology, Katowice, Poland 2. Warsaw University of Technology, Warsaw, Poland andrzej [email protected] Keywords: AJ62, magnesium alloy, long-term annealing, microstructure
The paper presents results of SEM investigations of AJ62 magnesium alloy in as cast condition and after long-term annealing. The AJ62 contains approximately 6% aluminum and about 2,5% strontium. The Mg-Al-Sr alloys exhibit good elevatedtemperature tensile properties, excellent creep resistance (better than Mg-Al-RE) and good castability [1]. The alloys have also Zn, Si And Mn. Strontium is added for creep resistance in die casting and gravity casting alloys or to reduced shrinkage porosity. Sr level may range from 0,02% to 3% [2]. The Mg-Al-Sr alloys (AJ52, AJ62) show different microstructure based on the Sr/Al ratio. For Sr/Al ratio below 0.3, the microstructure consists of α-Mg with precipitates of Al4Sr phase. When the Sr/Al ratio increases, a second intermetallic phase (probably Al3Mg13Sr) is observed together with Al4Sr phase. This ratio also controls the precipitation of Mg17Al12 phase. When Sr/Al ratio is very low this phase occur in the α-Mg matrix [3,4]. The material for the research was a sand casting AJ62 magnesium alloy. The chemical composition of this alloy is provided in Table 1. Sand casting was performed at 700°C temperatures. Annealing treatments were performed at 180°C, 250°C and 350°C during 500÷3000h with cooling in air. The microstructure of AJ62 alloy was examined by a Hitachi S3400 Scanning Electron Microscope. The AJ62 magnesium alloy after sand casting was characterized by the solid solution α with the lamellar eutectic (Al,Mg)4Sr + solid solution α and the globular precipitates of the Mn5Al8 phase. Morever the occurrence of not mumerous precipitates of the massive Al3Mg13Sr phase have been provided (Fig.1). Annealing this alloy at 180°C results the precipitation of Mg17Al12 phase and beginning of Al3Mg13Sr phase decomposition (Fig.2). Long-term annealing (3000h) at 250°C causes more far decomposition of Al3Mg13Sr phase (Fig.3). The precipitates of Mg17Al12 phase were not observed. Morphology and volume fraction of (Al,Mg)4Sr phase didn’t change. After exposure at 350°C the total decomposition of Al3Mg13Sr phase on mixture Al4Sr + αMg phases was observed (Fig.4). 1. 2. 3.
A.A.Luo, Materials Science Forum, Vols. 419-422, (2003), p. 57. H.E.Friedrich, B.L.Mordike, Magnesium Technology, Springer-Verlag Berlin Heidelberg, (2006). M.O.Pekguleryuz, Proc. 6th International Conference Magnesium Alloys and their Applications, Wolfsburg (2003), p.74.
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 441–442, DOI: 10.1007/978-3-540-85226-1_221, © Springer-Verlag Berlin Heidelberg 2008
442
4. 5.
B.Jing, S.Yangshan, X.Shan, X.Feng, Z.Tianbai, Materials Science and Engineering A419 (2006), p.181. The present work was supported by the Polish Ministry of Science and Higher Education under the research project No PBZ-KBN-114/T08/2004.
Table I. Chemical composition of the AJ62 magnesium alloy in wt.-%. Alloy
Mg
Al
Mn
Sr
AJ62
balance
6,1
0,34
2,1
Figure 1. Precipitates of (Al,Mg)4Sr and Figure 2. Beginning of Al3Mg13Sr phase Al3Mg13Sr phases in AJ62 alloy after sand decomposition and precipitates of Mg17Al12 casting. phase in AJ62 alloy after annealing at 180°C/1000h.
Figure 3. Decomposition of Al3Mg13Sr phase after 3000h exposure at 250°C.
Figure 4. Total decomposition of Al3Mg13Sr phase on mixture Al4Sr + α phases after 1000h exposure at 350°C.
443
EELS characterisation of the interface between nanoscaled ODS particles and matrix in advanced fusion steels M. Klimenkov, R. Lindau and A. Möslang Institute for Materials Research I, Forschungszentrum Karlsruhe GmbH Hermann-von-Helmholtz-Platz 1, 76344 Eggenstein-Leopoldshafen, Germany michael klimenkov@imf fzk.de Keywords: EELS, ODS steels, interfaces
Reduced activation ferritic–martensitic alloys (RAFM) are primary candidates for structural application in breeding blankets of fusion reactor plants, mainly due to their excellent swelling resistance and low activation properties. By the selection a of specific production route for ODS-Eurofer steel of the second generation, which included rolling and appropriate thermal treatments, DBTT could be shifted from values between +60 and +100°C for hipped ODS-Eurofer to values between -40 and -80°C° [1]. In addition ductility was improved significantly. This ductility improvement of the steel properties could be attributed to dislocation pinning on ODS particles. TEM examination of the ODS particle/matrix interface is a step toward understanding of the pinning mechanism and herewith the possibility to predict the steel properties. The TEM investigation of the ODS particle – matrix interfaces shows that ODS particles are in no case single Y2O3 phase dispersoids as it was suggested in the earlier publications [2]. The analytical TEM investigations using 1nm spatial resolution clearly show that all ODS particles have a complex shell/core structure (Figure 1). The Fe, Cr and Y - maps show, that the investigated Y2O3 ODS particle is imbedded in the matrix. The V-rich shell is clearly visible in the V-map. Performing spatially resolved EELS experiments clearly confirms the formation of a V rich shell around ODS particles (Figure 2). The intensity of the V-L2,3 edge increases at the edge of the ODS particle indicating a V-rich shell. The O-K edge shows the fine structure that is typical for Y2O3 material. The intensity of this edge is not zero in the regions outside the ODS particle due to the oxidation of specimen surface. Using the cross section scattering ratio of 1.8 for Mn-L2,3 and O-K EELS edges it was estimated, that the Mn/O ratio is about 0.05 to 0.10. From these considerations a (Y1 8Mn0 2)O3 composition of this ODS particle can be estimated. The earlier analytical investigations, which have been performed using EDX method did not detect Mn inside ODS particles because Mn-Kα and Mn-Kβ lines overlap with Cr-Kβ and Fe-Kα lines – the main alloying elements. The formation of thin oxide films on the specimen surface produces the weak O signal and disturbs herewith the typical energy loss near edge structure (ELNES) of measured spectra. This is especially important for the spectra obtained directly on the interfaces, where the ELNES fluctuations are very weak. From the spectra presented in the Figure 2 a “background” spectrum from the matrix was subtracted. The spectrum taken 1.5 nm from the interface in the matrix does not show any structure (Figure 3a)
S. Richter, A. Schwedt (Eds.): EMC 2008, Vol. 2: Materials Science, pp. 443–444, DOI: 10.1007/978-3-540-85226-1_222, © Springer-Verlag Berlin Heidelberg 2008
444
while the spectrum obtained directly on the interface (Figure 3b) shows V-L2,3 and O-K signals only. The signal from the Y2O3 core shows a strong O-K signal and Mn-L2,3 edge (Figure 3c). These difference spectra clearly show that the shell consists of V oxide. 1. 2.
R. Lindau, A. Moslang, M. Schirra, P. Schlossmacher, M. Klimenkov, Journal of Nuclear Materials 307-311 (2002) 769 M. Klimiankou, R. Lindau, A. Moslang Journal of Crystal Growth 249 (2003) 381
b)
c)
Fe
Cr
d)
e)
Y
V
a)
25nm
O-K
V-L2,3
Cr-L2,3
Mn-L2,3
1 .5
inte rfa c + e
+3.0
/nm
a)
-4.5
.5
Dis tan -3.0 ce fr -1 o m
0
b)
20 nm
500
30
600
Mn-L2 3
Figure 3. The interface spectra after subtraction of background spectrum from the surrounded matrix.
O-K
counts
Cr-L2,3 c)
20 10
V-L2,3 O-K
b) a)
0
550
600
Energy /keV
Figure 2. Spatially resolved EELS investigations of ODS particle /matrix interfaces. The area with two ODS particles is imaged in the part (a). The row of EELS spectra obtained while the scanning along the marked line is presented in part (b).
550
Energy /keV
650
650
Figure 1. EDX elemental mapping of an area with ODS particle: (a) shows the HAADF image, (b) – (e) represent the elemental maps obtained using Fe-Kα, Cr-Kα, Y-L, and V-Kα EDX lines respectively.
445
Microstructure-mechanical property relationships in a maraging 250 steel P. Kokkonidis, E. Papadopoulou, A. Rizos, T. Koutsoukis and G. Fourlaris Laboratory of Physical Metallurgy, National Technical University of Athens, 9 Heroon Polytechniou St. , 15780, Athens Greece pkokkoni@mail ntua.gr Keywords: maraging 250, microstructure, mechanical properties, ageing
The objective of the present study is to examine the relationship of the microstructure with its mechanical properties in a maraging 250 steel, following a series of selected ageing experiments. Furthermore, the effect of cold plastic deformation (cold rolling, at different amounts of cold rolling reduction) on the mechanical properties of the steel following ageing was also studied. Maraging steels represent a distinct family of high strength steels. They exhibit a characteristic strengthening sequence following a precipitation at 480 o C [1]. A typical characteristic of this family of steels is their combination of enhanced ductility with high tensile strength values. [2] The samples were initially solution treated at 820°C for 30mins followed by water quenching (room temperature). Aging took place at 460°C, or 480°C or 510°C for periods of time ranging from 30mins to 24h, followed by water quenching (20οC). For the microstructure investigation a scanning electron microscope (Philips XL30) was employed coupled with X-ray diffraction phase identification. The hardness of specimens was measured using a Vickers hardness testing facility. Finally, selective tensile testing was carried out in specimens that were aged at 510οC. The experimental results showed an increase in hardness at all three chosen ageing temperatures, even for the brief ageing time of 30 mins. Aged specimens were compared with specimens that were annealed at 820ο C for 30 min and quenched in water. Following prolonged ageing, a decrease in hardness was observed for ageing times of more than 24h at 510οC (Figure 1). Tensile testing confirmed the influence of ageing on the mechanical properties of this steel grade (Figure