ELECTROMAGNETIC NONDESTRUCTIVE EVALUATION (XI)
Studies in Applied Electromagnetics and Mechanics Series Editors: K. Miya, A.J. Moses, Y. Uchikawa, A. Bossavit, R. Collins, T. Honma, G.A. Maugin, F.C. Moon, G. Rubinacci, H. Troger and S.-A. Zhou
Volume 31 Previously published in this series: Vol. 30. Vol. 29. Vol. 28. Vol. 27. Vol. 26. Vol. 25. Vol. 24. Vol. 23. Vol. 22. Vol. 21. Vol. 20. Vol. 19. Vol. 18. Vol. 17. Vol. 16. Vol. 15. Vol. 14. Vol. 13. Vol. 12.
S. Wiak, A. Krawczyk and I. Dolezel (Eds.), Advanced Computer Techniques in Applied Electromagnetics A. Krawczyk, R. Kubacki, S. Wiak and C. Lemos Antunes (Eds.), Electromagnetic Field, Health and Environment – Proceedings of EHE’07 S. Takahashi and H. Kikuchi (Eds.), Electromagnetic Nondestructive Evaluation (X) A. Krawczyk, S. Wiak and X.M. Lopez-Fernandez (Eds.), Electromagnetic Fields in Mechatronics, Electrical and Electronic Engineering G. Dobmann (Ed.), Electromagnetic Nondestructive Evaluation (VII) L. Udpa and N. Bowler (Eds.), Electromagnetic Nondestructive Evaluation (IX) T. Sollier, D. Prémel and D. Lesselier (Eds.), Electromagnetic Nondestructive Evaluation (VIII) F. Kojima, T. Takagi, S.S. Udpa and J. Pávó (Eds.), Electromagnetic Nondestructive Evaluation (VI) A. Krawczyk and S. Wiak (Eds.), Electromagnetic Fields in Electrical Engineering J. Pávó, G. Vértesy, T. Takagi and S.S. Udpa (Eds.), Electromagnetic Nondestructive Evaluation (V) Z. Haznadar and Ž. Štih, Electromagnetic Fields, Waves and Numerical Methods J.S. Yang and G.A. Maugin (Eds.), Mechanics of Electromagnetic Materials and Structures P. Di Barba and A. Savini (Eds.), Non-Linear Electromagnetic Systems S.S. Udpa, T. Takagi, J. Pávó and R. Albanese (Eds.), Electromagnetic Nondestructive Evaluation (IV) H. Tsuboi and I. Vajda (Eds.), Applied Electromagnetics and Computational Technology II D. Lesselier and A. Razek (Eds.), Electromagnetic Nondestructive Evaluation (III) R. Albanese, G. Rubinacci, T. Takagi and S.S. Udpa (Eds.), Electromagnetic Nondestructive Evaluation (II) V. Kose and J. Sievert (Eds.), Non-Linear Electromagnetic Systems T. Takagi, J.R. Bowler and Y. Yoshida (Eds.), Electromagnetic Nondestructive Evaluation
Volumes 1–6 were published by Elsevier Science under the series title “Elsevier Studies in Applied Electromagnetics in Materials”. ISSN 1383-7281
Electromagnetic Nondestructive Evaluation (XI)
Edited by
Antonello Tamburrino University of Cassino, Italy
Yevgen Melikhov Cardiff University, UK
Zhenmao Chen Xian Jiaotong University, China
and
Lalita Udpa Michigan State University, USA
Amsterdam • Berlin • Oxford • Tokyo • Washington, DC
© 2008 The authors and IOS Press. All rights reserved. No part of this book may be reproduced, stored in a retrieval system, or transmitted, in any form or by any means, without prior written permission from the publisher. ISBN 978-1-58603-896-0 Library of Congress Control Number: 2008932761 Publisher IOS Press Nieuwe Hemweg 6B 1013 BG Amsterdam Netherlands fax: +31 20 687 0019 e-mail:
[email protected] Distributor in the UK and Ireland Gazelle Books Services Ltd. White Cross Mills Hightown Lancaster LA1 4XS United Kingdom fax: +44 1524 63232 e-mail:
[email protected]
Distributor in the USA and Canada IOS Press, Inc. 4502 Rachael Manor Drive Fairfax, VA 22032 USA fax: +1 703 323 3668 e-mail:
[email protected]
LEGAL NOTICE The publisher is not responsible for the use which might be made of the following information. PRINTED IN THE NETHERLANDS
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved.
v
Preface The 12th International Workshop on Electromagnetic Nondestructive Evaluation (ENDE’07) was held from 19th–21st June 2007. The Workshop was hosted by the Wolfson Centre for Magnetics at Cardiff University, Cardiff, Wales, UK with sponsorship from Cedrat SA, Serco Assurance, Rolls-Royce plc, Welsh Assembly Government, Computer Simulation Technology, The Japan Society of Applied Electromagnetics and Mechanics, Engineering and Physical Sciences Research Council. The organizers gratefully acknowledge their support. The aim of this annual workshop is to bring together engineers and scientists from universities, research institutions and industry to discuss and exchange the latest ideas and findings in basic research and development as well as industrial applications of Electromagnetic Nondestructive Evaluation. After the introductory welcoming remarks from Dr. David Grant (Vice Chancellor of the Cardiff University), Prof. Hywel Thomas (Head of the School of Engineering, Cardiff University) and Prof. David Jiles (Chairman of the Workshop), the technical program of the Workshop commenced with a plenary talk “NDE Research Makes a Difference” by Prof. Chris Scruby, Director, UK Research Centre in NDE, Imperial College London, U.K. Four distinguished invited speakers discussed the challenges and achievements in various fields of ENDE. Prof. J. Bowler (Iowa State University, USA), gave a talk titled “Integral methods for calculating the interaction of eddy currents with cracks”. Prof. K. Miya (Keio University, Japan), presented the second invited talk on “The Start of a New Field of Electromagnetic and Mechanical Maintenance Engineering”. Prof. G. Dobmann (Fraunhofer-Institute for Non-destructive Testing, Germany), was invited to present “Industrial Applications of 3MA – Micromagnetic Multiparameter Microstructure and Stress Analysis”. Finally Prof. N. Takahashi (Okayama University, Japan) presented an invited talk on “3D Nonlinear Eddy Current Analysis of Electromagnetic Inspection of Defects in Steel”. A total of 75 technical papers were divided into 30 oral and 45 poster presentations. The oral presentations were organized into 7 sessions covering a variety of topics on both theoretical and experimental aspects of NDE in eddy currents, magnetic measurements, magnetic flux leakage, Barkhausen methods, new methods and inverse problems for crack detection. These sessions were chaired by experts in the field including Profs. S. Udpa, L. Udpa, D. Jiles, C. Scruby, P. Nagy, T. Moses, G. Dobmann, K. Miya, S. Takahashi, A. Tamburrino and others. During closing remarks it was announced that the next ENDE Workshop (ENDE2008) will be held June 10–12, 2008 in Seoul, Korea. The ENDE Workshop 2009 will be held in Dayton, Ohio, U.S.A. The conference concluded with remarks from the chairman Prof. David Jiles. A total of 73 participants from 16 countries were registered for the Workshop. The short versions of the papers were published in the Workshop digest and 39 reviewed full papers were accepted for publication in this proceeding. The organizers would like to thank all the participants for their contribution and all the referees for their role in reviewing the full papers. Lastly, the editors gratefully acknowledge the help and hard work of Ms. Linda Clifford in putting this volume together.
This page intentionally left blank
vii
List of Referees J. Aldrin Z. Badics J. Bowler N. Bowler T. Chady M. Chan Z. Chen W. Cheng G. Dobmann Y. Gotoh R. Grimberg X. Hao H. Huang G. Hwang L. Janousek H. Kikuchi S. Kobayashi F. Kojima J. Lee D. Lesselier L. Li Y. Melikhov V. Melapudi O. Mihalache T. Moses G. Ni J. Pávó P. Ramuhalli G. Rubinacci O. Stupakov J. Taggart A. Tamburrino T. Takagi N. Takahashi S. Takahashi T. Theodoulidis G.Y. Tian I. Tomas Y. Tsuchida L. Udpa S. Udpa M. Vaidhianathasamy S. Ventre
Computational Tools, USA Rhythmia Medical, Inc, USA Iowa State University, USA Iowa State University, USA Technical University of Szczecin, Poland Michigan State University, USA Xi’an Jiaotong University, China Tsurumi R&D Center, JAPEIC, Japan Fraunhofer-IZFP University, Germany Oita University, Japan National Institute of R&D for Technical Physics, Romania University of Birmingham, United Kingdom IIU Corporation, Japan Shanghai Jiaotong University, China University of Zilina, Slovakia Iwate University, Japan Iwate University, Japan Kobe University, Japan Chosun University, Korea Supélec, France Tsinghua University, China Cardiff University, United Kingdom Michigan State University, USA JAEA, Japan Cardiff University, United Kingdom Zhejing University, China Budapest University of Technology and Economics, Hungary Michigan State University, USA Università degli Studi di Napoli “Federico II”, Italy Tohoku University, Japan Serco Assurance, United Kingdom University of Cassino, Italy Tohoku University, Japan Okayama University, Japan Iwate University, Japan University of Western Macedonia, Greece University of Newcastle upon Tyne, UK Institute of Physics, Czech Republic Oita University, Japan Michigan State University, USA Michigan State University, USA University of Newcastle Upon Tyne, United Kingdom University of Cassino, Italy
viii
M. Versaci F. Villone J. Wilson L. Xin N. Yusa Z. Zeng
Università “Mediterranea” di Reggio Calabria, Italy University of Cassino, Italy University of Newcastle Upon Tyne, United Kingdom Michigan State University, USA IIU Corporation, Japan Michigan State University, USA
ix
Organizing Committees International Committee Chairman
• S. Udpa, Michigan State University, USA
Members
• • • • • • • • • • • • • • • • • •
J.R. Bowler, Iowa State University, U.S.A. N. Bowler, Iowa State University, U.S.A. Z. Chen, Xian Jiaotong University, China G. Dobmann, Fraunhofer Institute for NDT, Germany H.K. Jung, Seoul National University, South Korea F. Kojima, Kobe University, Japan D. Lesselier, DRE-LSS CNRS-SUPELEC-UPS, France K. Miya, Keio University, Japan G.Z. Ni, Zhejing University, China J. Pavo, Budapest University, Hungary G. Pichenot, CEA SACLAY, France A. Razek, LGEP CNRS-SUPELEC-UPS-UPMC, France G. Rubinacci, Universita di Napoli Federico II, Italy S.J. Song, Sung Kwan University, Korea T. Takagi, Tohoku University, Japan S. Takahashi, Iwate University, Japan A. Tamburrino, Universita degli Studi di Cassino, Italy L. Udpa, Michigan State University, U.S.A.
Organizing Committee
• • • • • • • • •
Tony Dunhill, Rolls Royce Plc Keith Jenkins, Cogent Power David Jiles, Cardiff University (Chairman) Chester Lo, Iowa State University Tony Moses, Cardiff University Ian Nicholson, TWI Ltd Allan Rogerson, Serco Assurance Plc Chris Scruby, Imperial College London Gui Yun Tiann, University of Huddersfield
Local Committee
• • • • • •
Phil Anderson Jeremy Hall Eugene Melikhov John Snyder Paul Williams Stan Zurek
This page intentionally left blank
xi
List of Participants Mr. Kavoos Abbasi Tohoku University, Japan
[email protected]
Dr. Dagmar Faktorova University of Zilina, Slovak Republic
[email protected]
Prof. Purnachandra Rao Bhagi Indira Ghandi Centre for Atomic Research, India
[email protected]
Mr. Fabrice Foucher CEDRAT, France
[email protected]
Prof. John Bowler Iowa State University, USA
[email protected]
Dr. Raimond Grimberg National Inst. of R & D for Technical Physics, Romania
[email protected]
Dr. Nicola Bowler Iowa State University, USA
[email protected]
Dr. Xinjiang Hao Birmingham University, UK
[email protected]
Dr. John Burd JB Consulting Ltd, UK
[email protected]
Dr. Jeremy Hall Wolfson Centre for Magnetics, UK
[email protected]
Hee Jun Chen Sungkyunkwan University, Korea
[email protected]
Mr. Jiseong Hwang Chosun University, Republic of Korea
[email protected]
Dr. Zhenmao Chen Xian Jiaotong University, China
[email protected]
Dr. Richard Ireland QinetiQ, UK
[email protected]
Prof. Gerd Dobmann Fraunhofer-Institut IZFP, Germany
[email protected]
Dr. Ladislav Janousek University of Zilina, Slovak Republic
[email protected]
Mr. David Edgar University of Nottingham & Qinetiq, UK
[email protected]
Dr. Mohan Jayawardene CST, UK/Germany
[email protected]
Dr. Christiaan Eggink Shell Global Solutions Int., Netherlands
[email protected]
Dr. Steve Jenkins Current Enterprises, UK
[email protected]
xii
Prof. David Jiles Wolfson Centre for Magnetics, UK
[email protected]
Dr. Dmitriy Makhnovskiy University of Plymouth, UK
[email protected]
Dr. Tonphong Kaewkongka Chulalongkorn University, Thailand
[email protected]
Dr. Eugene Melikhov Wolfson Centre for Magnetics, UK
[email protected]
Mr. Yuchiro Kai Oita University, Japan
[email protected]
Prof. Kenzo Miya IIU, Japan
[email protected]
Dr. Hiroaki Kikuchi NDE & SRC Ueda, Japan
[email protected]
Prof. Tony Moses Wolfson Centre for Magnetics, UK
[email protected]+D70
Mr. Jeremy Knopp Air Force Research Laboratory, USA
[email protected]
Dr. Shoichiro Nagata University of Miyazaki, Japan
[email protected]
Dr. Satoru Kobayashi NDE & Science Research Centre, Japan
[email protected]
Prof. Peter BN Nagy University of Cincinnati, USA
[email protected]
Prof. Fumio Kojima Kobe University, Japan
[email protected] Dr. Yann Le Bihan LGEP- SUPELEC, France
[email protected] Prof. Jinyi Lee Chosun University, Republic of Korea
[email protected]
Severine Paillard CEA, France
[email protected] Dr. Manuele Papais University of Udine, Italy
[email protected] Dr. Grégoire Pichenot CEA, France
[email protected]
Dr. Yohan Le Diraison ENS-CACHAN, France
[email protected]
Mr. Grzegorz Psuj Szczecin University of Technology, Poland
[email protected]
Dr. Dominique Lesselier SUPELEC, France
[email protected]
Mr. Brian Radtke Iowa State University, USA
[email protected]
Prof. Li Luming Tsinghua University, China
[email protected]
Miss Alicia Romero Ramirez Swansea University, UK
[email protected]
xiii
Dr. Cyril Ravat ENS-CACHAN, France
[email protected]
Prof. Norio Takahashi Okayma University, Japan
[email protected]
Dr. Alan Rogerson Serco Assurance, UK
Prof. Seiki Takahashi Iwate University, Japan
[email protected]
Dr. Adriana Savin National Inst. of R & D for Technical Physics, Romania
[email protected]
Prof. Antonello Tamburrino Daeimi University of Cassino, Italy
[email protected]
Prof. Chris Scruby Imperial College, UK
[email protected]
Dr. Alan Tassin ENS-CACHAN, France
[email protected]
Dr. Gongtian Shen CSEI, China
[email protected]
Dr. Theodoros Theodoulidis University of West Macedonia, Greece
[email protected]
Prof. Young-Kil Shin Kunsan National University, South Korea
[email protected]
Prof. Gui Yun Tian Newcastle University, UK
[email protected]
Dr. Anastassios Skarlatos CEA, France gregoire.pichenot.cea.fr
Mr. Yuji Tsuchida Oita University, Japan
[email protected]
Dr. Sung-Jin Song Sungkyunkwan University, Korea
[email protected] Mr. Giuseppe Sposito Imperial College, UK
[email protected] Dr. Vladamir Syasko Constanta, Russia
[email protected] Dr. John Taggart Serco Assurance, UK
[email protected] Prof. Toshiyuki Takagi Tohoku University, Japan
[email protected]
Dr. Lalita Udpa Michigan State University, USA
[email protected] Prof. Satish Udpa Michigan State University, USA
[email protected] Dr. Tetsuya Uchimoto Tohoku University, Japan
[email protected] Dr. Moorthy Vaidhianathasamy Newcastle University, UK
[email protected] Dr. Haitao Wang Nanjing University of Aeronautics & Astronautics, China
[email protected]
xiv
Dr. Casper Wassink Applus RTD, The Netherlands
[email protected]
Mr. John Wilson Newcastle University, UK
[email protected]
Mr. Chris Ward University of Nottingham/RWE NPower, UK
[email protected]
Mr. Chen Xing Tsinghua University, China
[email protected]
Dr. Paul Williams Wolfson Centre for Magnetics, UK
[email protected]
Dr. En Tao Yao Nanjing University of Aeronautics & Astronautics, China
[email protected]
xv
Contents Preface
v
List of Referees
vii
Organizing Committees
ix
List of Participants
xi
Invited Speakers A Start of New Field of Electromagnetic and Mechanical Maintenance Engineering Kenzo Miya NDE Research Makes a Difference C.B. Scruby
3 10
Industrial Applications of 3MA – Micromagnetic Multiparameter Microstructure and Stress Analysis Gerd Dobmann, Iris Altpeter, Bernd Wolter and Rolf Kern
18
3D Nonlinear Finite Element Analysis of Electromagnetic Inspection of Defects in Steel N. Takahashi and Y. Gotoh
26
Magnetic Materials Evaluation of Irradiation Embrittlement in Fe-Cu-Ni-Mn Model Alloys by Measurements of Magnetic Minor Hysteresis Loops Satoru Kobayashi, Hiroaki Kikuchi, Seiki Takahashi, Katsuyuki Ara and Yasuhiro Kamada Analysis of Barkhausen Noise Characteristics and Mechanical Properties on Cold Rolled Low Carbon Steel Hiroaki Kikuchi, Tomoki Koshika, Tong Liu, Yasuhiro Kamada, Katsuyuki Ara, Satoru Kobayashi and Seiki Takahashi A Bridge Between NDE and Charpy Impact Testing Seiki Takahashi and Satoru Kobayashi ND-Materials Characterization of Neutron-Induced Embrittlement in German Nuclear Reactor Pressure Vessel Material by Micromagnetic NDT Techniques Gerd Dobmann, Iris Altpeter, Melanie Kopp, Magdalena Rabung and Gerhard Hübschen Evaluation of Chill Contents in Flake Graphite Cast Irons Using AC Magnetization Method Tetsuya Uchimoto, Jun Matsukawa, Toshihiko Abe, Toshiyuki Takagi, Takeshi Sato, Hiroyuki Ike, Takahito Takagawa and Noritaka Horikawa
37
42
46
54
62
xvi
Characterisation of Microstructures in Heat Treated Maraging Steel Using Eddy Current and Barkhausen Emission Techniques K.V. Rajkumar, B.P.C. Rao, B. Sasi, S. Vaidyanathan, T. Jayakumar and Baldev Raj
70
Novel Acoustic Barkhausen Noise Transducer and Its Comparison with Electromagnetic Acoustic Transducer John Wilson, Gui Yun Tian, Rachel S. Edwards and Steve Dixon
78
Modelling and Measurement of Decarburisation of Steels Using a Multi-Frequency Electromagnetic Sensor X.J. Hao, W. Yin, M. Strangwood, A.J. Peyton, P.F. Morris and C.L. Davis
86
Assessment of Grinding Damage on Gear Teeth Using Magnetic Barkhausen Noise Measurements Moorthy Vaidhianathasamy, Brian Andrew Shaw, Will Bennett and Peter Hopkins Evaluation of Contact Fatigue Damage on Gears Using the Magnetic Barkhausen Noise Technique Moorthy Vaidhianathasamy, Brian Andrew Shaw, Will Bennett and Peter Hopkins
90
98
Inverse Problems 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections Alessandro Pirani, Marco Ricci, Antonello Tamburrino and Salvatore Ventre
109
Multi-Frequency Eddy Current Imaging for the Detection of Buried Cracks in Aeronautical Structures Yohan Le Diraison and Pierre-Yves Joubert
117
A Comparative Study of Source Separation Techniques for the Detection of Buried Defects in the EC NDE of Aeronautical Multi-Layered Lap-Joints Alan Tassin, Yohan Le Diraison and Pierre-Yves Joubert
125
Fundamental Feature Extraction Methods for the Analysis of Eddy Current Data Jeremy S. Knopp and John C. Aldrin
133
Inversion of Potential Drop Data for the Reconstruction of Crack Depth Profiles Giuseppe Sposito, Peter Cawley and Peter B. Nagy
141
Automatic Classification of Defects with the Review of an Appropriate Feature Extraction Alicia Romero Ramirez, Neil Pearson and J.S.D. Mason
148
Microwave Nondestructive Detection of Longitudinal Cracks in Pipe with U-Bend and Prediction of Its Location by Signal Processing Kavoos Abbasi, Satoshi Ito and Hidetoshi Hashizume
154
Some Experiences with Microwave Investigation of Material Defects Dagmar Faktorová
162
xvii
Modeling Effect of Crack Closure on Quantitative ECT Inspection of Closed Fatigue Cracks Zhenmao Chen, Noritaka Yusa, Kenzo Miya and Hideaki Tokuma Toward the Reconstruction of Stress Corrosion Cracks Using Benchmark Eddy Currents Signals Maxim Morozov, Guglielmo Rubinacci, Antonello Tamburrino, Salvatore Ventre and Fabio Villone Evaluation of Subsurface Cracks in Riveted Aluminium Joints Using Industrial Eddy Current Instrumentation Maxim Morozov, Guglielmo Rubinacci, Antonello Tamburrino and Salvatore Ventre Design of a System for the Long Defects Detection with Advanced Methods for Eddy-Currents Analysis E. Cardelli, A. Faba, A. Formisano, R. Martone, F.C. Morabito, M. Papais, R. Specogna, A. Tamburrino, F. Trevisan, S. Ventre and M. Versaci
171
179
187
195
Theory of Four-Point Alternating Current Potential Drop Measurements on a Layered Conductive Half-Space Nicola Bowler and John R. Bowler
203
Integration of Tilted Coil Models in a Volume Integral Method for Realistic Simulations of Eddy Current Inspections Theodoros Theodoulidis and Gregoire Pichenot
211
Modeling of Flawed Riveted Structures for EC Inspection in Aeronautics S. Paillard, G. Pichenot, Y. Choua, Y. Le Bihan, M. Lambert, H. Voillaume and N. Dominguez Numerical Modeling of Eddy Current Nondestructive Evaluation of Ferromagnetic Tubes via an Integral Equation Approach Anastassios Skarlatos, Grégoire Pichenot, Dominique Lesselier, Marc Lambert and Bernard Duchêne Design of Reflection Type Pulsed Eddy Current Nondestructive Testing Young-Kil Shin, Dong-Myung Choi and Hee-Sung Jung
217
225
231
Applications Noninvasive Characterization of Bjork-Shiley Convexo-Concave Prosthetic Heart Valves Using an Electromagnetic Method Raimond Grimberg, Shiu C. Chan, Adriana Savin, Lalita Udpa and Satish S. Udpa Remote Field Eddy Current Control Using Rotating Magnetic Field Transducer. Application to Pressure Tubes Examination Adriana Savin, Lalita Udpa, Rozina Steigmann, Alina Bruma, Raimond Grimberg and Satish S. Udpa
241
249
xviii
Lifetime Prediction of Pressure Tubes in PHWR Nuclear Power Plants Using Eddy Current Data Raimond Grimberg, Adriana Savin, Rozina Steigmann, Aurel Andreescu, Nicoleta Iftimie and Marius Mihai Cazacu Electromagnetic Non-Destructive Evaluation of Reinforced Concrete Rebars Maxim Morozov, Guglielmo Rubinacci, Antonello Tamburrino and Salvatore Ventre
257
263
Advanced Probe with Array of Pick-Up Coils for Improved Crack Evaluation in Eddy-Current Non-Destructive Testing Ladislav Janousek, Klara Capova, Noritaka Yusa and Kenzo Miya
271
Observation of Stress Loaded Ferromagnetic Samples Using Remanent Flux Leakage Method Tomasz Chady, Grzegorz Psuj and Ryszard Sikora
276
Evaluation of Complex Multifrequency Eddy Current Transducer Designed for Precise Flaw Depth Measurements Tomasz Chady, Piotr Baniukiewicz, Ryszard Sikora and Grzegorz Psuj
283
Comparative Study of Coil Arrangements for the EC Testing of Small Surface Breaking Defects Cyril Ravat, Yann Le Bihan, Pierre-Yves Joubert and Claude Marchand
288
Author Index
295
Invited Speakers
This page intentionally left blank
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-3
3
A Start Of New Field Of Electromagnetic And Mechanical Maintenance Engineering Kenzo MIYA1 IIU, Corp., 2-7-17-7F, Ikenohata, Taitoku, Tokyo, 110-0008, Japan
Abstract. Maintenance to ensure the integrity of structures is one of the most important issues in modern industry, but more so in the nuclear power industry. This is primarily because complete prevention of all degradation of industrial materials is not possible, at least not in a realistic way. Consequently it is extremely important to detect degradation before machines start to loose their ability to function which may lead to harmful failures. Usually there is some kind of significant interval between the start of material degradation and failure; in other words, degradation usually progresses slowly with time. The problem is whether we can detect precursors of failure in the interval or not. If it is possible, we can have economic as well as safety related benefits because we are able to stop the machine before a functional failure and prevent an accident initiated by the failure of the machine. The benefits are not restricted to the nuclear power industry because it can be applied to any other heavy industry. There are many reasons why many conferences, such as ENDE, have been established to discuss and promote the progress of nondestructive inspection techniques. Whereas nondestructive inspection plays an important role in maintaining structural integrity and the performance of nondestructive inspection techniques should be enhanced in that sense, we need to regard it as one of several components composing “maintenance engineering.” Moreover, although nondestructive inspection is a proactive measure of maintenance, it is not a predictive tool. In fact, it is effective for detecting existing defects and does not say anything about the temporal evolution of defects. On the other hand, a condition monitoring system can offer significantly more useful information as mentioned above. In this paper I would like to introduce the concept of maintenology as a new science and technology in contrast to conventional maintenance engineering and to present several important results on electromagnetic maintenance for nuclear power plants as condition monitoring techniques (CMT). In particular, the introduction of electromagnetic maintenance is expected to play a very promising role in abnormality predictions of many dynamic machines that are required to be inspected regularly by law. Application of the technique would change conventional wisdom in thinking that machines should be taken apart and inspected regularly based on regulations. In many cases, this TBM (time based maintenance) is not too conservative in achieving an optimal maintenance approach.
Introduction The nuclear energy renaissance is occurring not only in advanced countries but also in developing ones like China, India and Brazil, due to demands for renewable energy sources and to protect the earth against abnormal climate caused by the green house effect. Nuclear power plants are one of the greenest sources of energy, and operated
4
K. Miya / A Start of New Field of Electromagnetic and Mechanical Maintenance Engineering
safely, can provide energy reliably to meet base loads. Thus, there is considerable interest in the safe and economic operation of nuclear power plants (NPPs). Maintenance engineering is extremely important to achieve these two goals. Two approaches are usually pursued: time-based maintenance (TBM) and condition-based maintenance (CBM). Optimal maintenance may be achieved by planning the best mix of the two approaches. The development of CBM techniques is greatly needed to enhance the safety level of NPPs. In this paper we explain the possibility of using electromagnetic methods and the application of the technology to maintenance operations at NPP. The essential part of electromagnetic maintenance technology is the utilization of u x B electromagnetic motive force (u: vectored velocity, B: magnetic field). In principle, diagnostics based on the technique can be applied to rotating machines at present although application could be extended to static components in future. Theoretical issues underlying the approach and experimental work associated with electromagnetic maintenance will be introduced first. Numerical simulations and experiments will then be presented.
1. Construction of maintenance engineering as a new field Maintenance issues comprise two different aspects, one is related to human behaviour and another relates to technical matters. Complicated human behaviour relating to maintenance of machines is considered to consist of three principles, as shown in Figure 1: the selection principle, connection principle and projection principle. Their relationship can be understood well if we imagine a process of making a sentence where proper words are selected first (selection principle), words are properly arranged to meet grammatical requirements (connection principle), and the intended meaning is realized by the sentence. The grammatically correct arrangement of words is called a projection principle. Concept of such a view is translated into maintenance activities like words corresponding to various kinds of technology supported by natural science, sociology, codes and standards, the connecting principle corresponding to maintenance scheme, and projection principle corresponding to the selection of necessary techniques from existing technological systems. These basic principles should be favourably applied to planning the maintenance scheme. In Fig. 2, a flow chart of maintenance activities is shown schematically. They start from the selection of the component to be maintained followed by the selection of the maintenance method, i.e. TBM or CBM, and then finally we proceed to the inspection process. This, in general, is the most universal process. In Fig. 3, concepts of maintenology are newly defined and explained to introduce a new approach to conventional maintenance engineering. The new approach consists of three principles depicted in Fig. 1; the basic form of maintenance action is shown in Fig.2. This recognition may contribute to the construction of revised maintenance engineering by applying theoretical aspects.
2. Electromagnetic maintenance engineering Principles of electromagnetic maintenance may be called the EM method. It is associated with the following processes: 1) Creation of a static magnetic field in a region of rotating components
5
K. Miya / A Start of New Field of Electromagnetic and Mechanical Maintenance Engineering
2) Measurement of a dynamic magnetic field created by eddy currents 3) Diagnosis of conditions of rotating parts inside, which can not be observed from the outside 4) Understanding the precursor of component abnormalities Measurements were carried out for real pumps, real fans, bearings, generating motors, etc. It was surprising to observe signals through thick casing of components overcoming the skin effect due to very low frequency. Simulation software was developed to predict eddy current distribution in components allowing one to judge whether conditions are normal or abnormal. This is a classical inverse problem but a very difficult one to solve due to ill-posedness. Ԙ Selection Principle
ԙ Projection principle
Ԛ Connection principle
System s
Component
㪪㫋㫉㫌㪺㫋㫌㫉㪼
ԘSelection of applicable engineering theories
Equipments
ԙReflection ԙReflection of maintenance technology on planning
Select appropriate technical knowledge from the engineering science system Codes&standards Sociology, economy Engineering science
Maintenanology
humanities
Ԛmaintenance scheme= Flow of maintenance activities
A-B-C-D-E-F…
Three elements of maintenance
1RGTCVKQP
Corrective actions
Characteristics of Aging (predictable㧛 unpredictable)
ԙAnalysis Evaluation Check Evaluation Investigations of root causes
Natural science
Component attribution Design Operation
+PUGTXKEG
ԚActions/Measures
ԘUnderstand the current state Inspections Tests Monitoring
㪘㪾㫀㫅㪾㩷㫆㪽㩷㪪㪪㪚
Maintenance engineering
Nuclear facilities
㪧㪸㫉㫋㫊
Classifications of maintenance methods Options
Logic of choice for maintenance methods
Inspection plans
Maintenance methods : Decomposition testing : Nondestructive testing : Function tests : Condition monitoring : Corrective Maintenance
Safety Safety Operation Operation
Figure 1. Principles underlying maintenance activities Maintenance Maintenance Engineering 1. 2. 3. 4. 5.
Maintenance Engineering
Maintenance Science Maintenance Engineering & Technology Maintenance Sociology M ethodology of optimization Codes and Standards development
Figure 2. Flow Chart of Maintenance
Theoretical Approach 1. 2. 3. 4. 5.
Theoretical Approach
Internal form of maintenance activities Basic form of maintenance action Academic development Application of P-D-C-A Theory of code and standard
Figure 3. Structure of maintenology
Figure 4. Eddy current distribution in blades (The largest eddy current will be generated in the area of the blade near the exciting coil. Due to this, magnetic flux changes in the direction coil are large. The excitation flux is constant and is not measured)
Casing
Impeller
Blades
Figure 5. Impeller model and meshes
Figure 6. Eddy current in ball bearings
K. Miya / A Start of New Field of Electromagnetic and Mechanical Maintenance Engineering
5.00E-07
Left scale for 5mm
4.00E-07
U (v)
3.00E-07
U: 5mm U: 10mm U: 15mm
5.00E-08
5.00E-07
4.00E-08
4.00E-07
5.00E-08
Left scale for 5mm
U: 5mm U: 10mm U: 15mm
4.00E-08
3.00E-08
3.00E-07
2.00E-07
2.00E-08
2.00E-07
2.00E-08
1.00E-07
1.00E-08
1.00E-07
1.00E-08
0.00E+00
0.00E+00
0.00E+00
0.00E+00
-1.00E-07
-1.00E-08
㧔V)-1.00E-07
-1.00E-08
-2.00E-07
-2.00E-08
-2.00E-07
-2.00E-08
-3.00E-07
-3.00E-08
-3.00E-07
-3.00E-08
-4.00E-07
-4.00E-08
-4.00E-07
-5.00E-07
-5.00E-08 0.02
-5.00E-07
㧔V)
0
0.002 0.004 0.006 0.008
0.01
0.012 0.014 0.016 0.018
U (v)
6
3.00E-08
-4.00E-08
0
0.002 0.004 0.006 0.008
Time(s)
0.01
0.012 0.014 0.016 0.018
-5.00E-08 0.02
Time(s)
With a holder
Without a holder
Figure 7. Signals from sensor. (1. Decrease of signal amplitude by 1/10 when distance becomes longer, from 5 to 10 mm. 2. Effect of a holder on signal is not significant, about 10% decrease) 3.00E-08 2.00E-08
U (v)
1.00E-08 0.00E+00 -1.00E-08 -2.00E-08
U: crack free U: V carck U: H crack
-3.00E-08 -4.00E-08 0
0.002
0.004
0.006
0.008
0.01
0.012
0.014
0.016
0.018
0.02
Time(s)
Figure 8. Ball bearings with a defect
Figure 9. Signals from defect
In Figure 4, four blades rotate around an axis which is not shown in the static magnetic field created by a permanent magnet (not shown here). Eddy current distribution induced in blades is shown in the figure together with a pick-up coil. If a crack is present or the blade is greatly deformed, we measure some changes in signals when abnormalities are present. In Figure 5 the finite element mesh for the impeller of a pump is shown. The finite element method is employed to evaluate eddy currents in the impeller. In Figure 6 ball bearings witness an orbital motion. The rotational eddy current is not significant, but the orbital motion produces a considerable amount of eddy currents in the balls. Thus, defects in a ball bearing may be easily detected by the method. If worn particles are present between bearings and steel plates, the speed of the orbital motion will change and this change can be detected using this method. Simulation results are shown in Fig. 7 for two cases: one is without a holder and the other is with a holder. Eddy currents in these cases are not different from each other indicating small effects of the holder. In the figure, “U” is a measure of distance between a bar magnet and surface of a casing. The measured signals largely depend on the distance, which is easily estimated by the decrease in the field due to the distance. The number of signal oscillations corresponds to the number of blades. In Fig. 8, the possibility of the detection of two notches on the surface of balls was tested by numerical simulation. The notches are in horizontal and vertical direction as shown in the figure. Results are shown in Fig.9. In the case of the vertical notch, differences from the case without a notch are evident but are difficult to find. This result can be explained from the magnitude of eddy currents due to positional differences of the two notches. Therefore, it becomes essentially important to optimize the relative position of a magnet and rotating blade.
K. Miya / A Start of New Field of Electromagnetic and Mechanical Maintenance Engineering
7
3. Experimental results The numerical results above were introduced on the basis of the explained concept to apply electromagnetic phenomena to defect inspection of rotating machines. The numerical results showed that there is a valid basis for the concept. The next step is to show experimental verification of the concept. Up to now, our research group has conducted many experiments with a small fans and pumps. We have also measured electromagnetic signals generated by rotating parts of real machines. When we can set a sensor and magnet close to the rotating parts, we can successfully measure a signal. However, when access is limited, it is difficult to obtain a useful signal. In Fig.10, measurement results are shown for the case of a fan. The signals were obtained as a function of distance between the sensor and the rotating part. When the distance is 5 mm, the signal is the largest and in the case of 20mm distance, the signal is the smallest. These results are from the set-up without fan casing. But, the 20mm distance result indicates that the measurement with a set-up that includes fan casing is possible. Results with the casing are not shown here, but a sufficient number of signals were obtained. Cyclic signals are obtained for 5 blades. There is the possibility that the smaller signal on the inside is due to a weight. The major purpose of this study is to verify the possible application of electromagnetic phenomena to proactive detection of various types of defects. Extensive studies must be conducted to find useful relations between signal changes and the condition of defects. Useful information must be provided to make engineering decisions on whether operation of the machine should be stopped for repair or continued with careful monitoring. With this in mind, we carried out an experiment with a notched blade as shown in Fig. 11. Two curves are shown corresponding to two types of bar and U-magnets. It is possible to see the movement of the 5 blades from both results. One of the blades was machined with the notch and signals reflecting an existence of the notch are observed in both results. Through a two-way excitation method, a crack of 1/3 the width was easily detected. Significant differences in signals were seen for cracks 1/10 the width. In Fig.12, three pictures of a casing of the real pump, location of a sensor and a pick-up coil, and an impeller are shown. The casing is cast iron and shows magnetic property. The rod type permanent magnet is attracted to the casing. 0.08
0.06 0.04 0.02 5mm 10mm 15mm 20mm
0
-0.02 -0.04 -0.06 -0.08 -2.00E-02 -1.50E-02 -1.00E-02 -5.00E-03 0.00E+00
Figure 10. Fan experiment
5.00E-03
1.00E-02
1.50E-02
2.00E-02
8
K. Miya / A Start of New Field of Electromagnetic and Mechanical Maintenance Engineering
1
1.5 Uဳ
1
0.8
ဳ
0.6 0.4
0.5 0.2 0
0
-0.2
-0.5
-0.4 -0.6
-1
-0.8
-1.5 -2.00E-02 -1.50E-02 -1.00E-02 -5.00E-03 0.00E+00 5.00E-03 1.00E-02 1.50E-02 2.00E-02
-1 -2.00E-02 -1.50E-02 -1.00E-02 -5.00E-03 0.00E+00 5.00E-03 1.00E-02 1.50E-02 2.00E-02
Figure 11. Detection of a defective blade
In Fig. 13, measurement results are shown. A careful examination shows that the number of impellers is 5 and the rotation cycle is 0.02 seconds since a motor operates at 50 Hz in the Kanto area in Japan. In addition to this, we can recognize a small difference in the amplitude of the measured voltage corresponding to the difference in size of the 5 blades. Since the signal amplitudes are different this suggests that the method can be applied to test for the dimension of axis and impellers, as well as their condition of motion. The wave form is not sinusoidal and shows a small tooth. The reason for the tooth is not clear until we see the inside of the pump after opening the casing. This small observation indicates that the detailed structure inside a rotating machine will be made clear after we accumulate knowledge on dimensional information and defects signals in the future.
Figure 12. Casing and impellers (real pump)
K. Miya / A Start of New Field of Electromagnetic and Mechanical Maintenance Engineering
9
Blade intervals are 0.004s 2 1.5 1
㔚䋨v䋩
0.5 0 -0.010
-0.005
0.000
0.005
0.010
0.015
0.020
0.025
0.030
0.035
0.040
-0.5 -1 -1.5 -2
Rotation cycles are 0.02s ᤨ㑆䋨s䋩
Figure 13. Signal with rod type permanent magnet sensor
3. Conclusion The author would like to note that there are many challenging problems in the diagnostics of rotating machines and that there is a strong need for developing methods of detecting abnormality precursors as a prognosticator of functional failure. There are well-known methods of condition monitoring. These include vibration monitoring methods, oil analysis, thermography, etc. These methods will be useful if they are used properly; however, there are several important problems to be solved in identifying the root causes of malfunctions occurring in a machine. Electromagnetic methods have shown their superiority over conventional methods in being able to locate defects and in identifying conditions at specific locations in rotating parts. Extensive studies are required to establish the relationship between the measured signal and the nature of defects. Efforts are urgently needed to translate R&D efforts to industrial applications.
10
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-10
NDE Research Makes a Difference C B SCRUBY UK Research Centre in NDE, Imperial College London, SW7 2AZ UK
Abstract. This paper discusses the development of research in NDE and its impact on industry. Examples will be given of past research projects that have been translated into solutions to industrial inspection problems, and present day challenges to industry and the NDE research community. Recurring themes include the need for quantification, and physical models to give scientific understanding and hence improved confidence for product quality and safetycritical application. Timely technology transfer is a continuing challenge and lessons from past experience will be discussed. Finally, the author will discuss future research strategy, including opportunities for interdisciplinary collaboration in order to integrate NDE more effectively into the engineering life cycle. Keywords. Non-destructive evaluation, NDE, electromagnetic.
Introduction There has been steady growth in non-destructive evaluation (NDE) research since the 1950s, reflecting the increasing demand for greater safety and environmental protection by the public. NDE research has always been particularly challenging. Firstly, the NDE field makes use of multiple technologies & disciplines, including magnetic, electrical, ultrasonic, radiographic, optical, and thermographic methods. Secondly, NDE is used for a wide range of materials (from metals to plastics, ceramics and composites) & applications (manufacturing process control, in-service inspection, defect sizing, corrosion measurement, and degradation monitoring). NDE is used in most sectors of industry: aerospace, power, oil & gas, transportation, infrastructure, built environment, manufacturing, nuclear, process, defence, electronics, packaging, etc., which have vastly different products and assets to be inspected – everything from electronic devices and foodstuffs through to entire rail networks and huge refineries. To enhance the challenge there is a complex supply chain to take new technologies from university research through to routine use, involving research and technology organizations (RTOs), service companies, equipment suppliers, certification and standards authorities, trainers and consultants (Figure 1). However, on the positive side, there is much commonality and overlap at the research stage in terms of techniques and generic applications. Many universities and RTOs have begun to recognize the benefits of an interdisciplinary approach to NDE research. Until the late 1980s much research was funded by government research laboratories and state-owned industries, especially in the nuclear and defence sectors. There were then changes due to privatisation that made a major impact on the funding of NDE research. Although the value of an NDE solution to an individual company or single industry sector may be too small to justify large investment, there are significant opportunities for collaborative funding to increase benefit, share risk and reduce cost.
C.B. Scruby / NDE Research Makes a Difference
Technique development
Service suppliers
Product development
Equipment suppliers
11
Asset owners and operators
Research
Product Manufacturers
Figure 1. The technology supply chain for NDE
Furthermore, generic research may attract government funding through its research councils, while pre-competitive, inter-sectoral, research collaborations lever public funding via for instance EU’s Framework Programmes. There are several key common themes affecting the effective application of NDE, and which are the drivers for research in NDE. The major ones are: coverage, overall inspection speed, quality of information delivered (sensitivity, accuracy, resolution, etc), accessibility of region to be inspected, reliability of the NDE measurement, applicability to a wide range of damage processes, materials and applications, reducing the need for skilled operator intervention (which implies autonomous inspection or monitoring systems), and of course the reduction of costs of the whole NDE process. The UK Research Centre in NDE (RCNDE) has a wide portfolio of NDE research within most of these theme areas.
1. The Research & Innovation Process for NDE The innovation process for NDE is no different from any other area of technology. Strong relationships in the supply chain (Figure 1) aid idea generation. As Figure 2 shows, there is usually some pioneering or opportunistic research before a more substantial research programme is undertaken. This is often followed by trials to evaluate the likely industrial benefits of the research. Depending upon the outcome, this may be followed by further, more applied research and development. If successful the new technology needs to be transferred or “translated” from research into product, a crucial and vulnerable step that will be discussed again. Commercialization, involving development of a market and sales, follows. However, development of the full potential of a product (or service), market penetration and acceptance, tends to be hindered if the technology is not embodied into standards and routine inspection procedures. Note that both scientific “push” and industrial “pull” are needed to drive this process; they need to overlap to ensure successful innovation. For a variety of reasons product development and commercialization sometimes accelerates beyond what can be supported by the market or the scientific foundation. As a result the technology is oversold which may lead to disillusionment. The only way forward is a realistic evaluation of both the underlying science and the proposed market, followed (if the conclusion is positive) by further research, development, optimization of the product to match industrial requirements, and hence through standardization into market acceptance.
12
C.B. Scruby / NDE Research Makes a Difference
230
Acceptance
Standardisation Commercialisation Product development 100 Further research & development
Trials & evaluation Research Pioneers 1
Technology development
121
-30
Scientific push Industrial pull
Figure 2. Research and innovation process for NDE
Within the defence and aerospace sectors of industry the innovation process is often described in terms of technology readiness levels (TRLs), as shown in Figure 3. Here the inventive phase is described as technology assessment. This may take place in an industrial R&D laboratory or an university. Production implementation is the remit of the end-user company. The challenge is the intermediate steps from 4 to 7; there is a need not only for organizations to undertake work at TRLs 5 and 6, but also to interact effectively with the organizations who carry out TRLs 1-4 on the one hand and TRLs 7-9 on the other. Experience has shown that the most risky part of the process is this translation from research to production. This may be because research and production are carried out by organizations with different objectives and cultures. The NDE industry has a relatively complicated supply chain for new technology (Figure 1) because the technology is used in both production and operation, and operators often sub-contract to service companies. There need to be routes to market for NDE services as well as products. In either case, improved ways are needed to facilitate the movement of new technology from left to right along the chain.
2. Case Studies of NDE Research and Innovation There are many potential examples within the field of electromagnetic NDE, but only a small number can be examined here with a view to understanding the process whereby a research idea is converted into an industrial technology. The examples are selected from the knowledge and experience of the author, and selection or omission is not a value judgment of the product in question. Alternating Current Field Measurement (ACFM) [1] is a current perturbation technique related to, but different from eddy current testing methods. Its development followed closely the pattern described by Figure 2. Thus there was scientific push in the form of university research at University College London (UCL) including
13
C.B. Scruby / NDE Research Makes a Difference
Proven Method
9. Track record established through successful applications 8. Production system qualified through test and demonstration
7. System prototype demonstration in an operational environment
6. Inspection optimised for capability and speed
Pre-Production
5. Inspection validated in relevant environment (prototype equipment)
4. Inspection validated in laboratory environment
Technology Assessment and Proving
Development
Production Implementation
3. Experimental proof of concept completed 2. Technology concept or application vetted or demonstrated 1. Basic principles observed and reported
Idea
Figure 3. Innovation process described in terms of Technology Readiness Levels
substantial modelling from 1987-9. This was followed in 1991 by application trials on model offshore nodes supported in part by the oil & gas industry, demonstrating growing industrial pull. In 1993 ACFM was licensed to TSC (a small university spinout company), with (1993) a royalty agreement to cover the UCL developments needed to commercialize the technology. 1994-8 saw the development of an applications market, mainly in oil & gas sector. This was supported by applications R&D in both university and company (1996-2000) with strong industrial pull. Standards for ACFM were published in 2003, and from 2004 onwards the focus was growing the application market and moving into the rail and nuclear sectors as the technology gained acceptance. The development was over a shorter period than some other examples, initial research to standard taking some 16 years. This was perhaps partly because the risk was reduced by the existence of an established market for eddy current technology. There was a good combination of scientific push and industrial pull for most of the development phase. But also, significantly, a strong supply chain based on close organizational and individual relationships was established early on. A second example is Pulsed Eddy Currents (PEC). It is based upon pioneering research at Argonne National Laboratory (USA) in 1950 with nuclear applications in mind. It was then picked up by the aerospace industry for detecting cracks in aluminium. In 1987 PEC was adapted by ARCO in their TEMP instrument (a pulsed eddy current device) to detect steel corrosion under insulation (CUI) for the oil and gas industry. In 1990 TEMP was licensed to RTD in Holland, being commercialized as INCOTEST. In 1994 Shell investigated PEC for detecting CUI, but found some shortcomings. However, at the same time, Shell carried out a laboratory investigation of PEC for other industrial applications. This led in 1996 to the launch of a commercial PEC system for a range of oil and gas applications, such as corrosion under fireproofing. There are no standards for PEC at the time of writing. The research from the 1980s onwards mainly took place in companies rather than universities, which ensured a strong industrial pull through most of development of PEC and a good potential market, once the target applications had been identified [2]. Basic research into eddy currents was started at RAE Farnborough (MoD) in collaboration with Surrey University in the 1970s. In the 1980s this moved on to eddy
14
C.B. Scruby / NDE Research Makes a Difference
current research using Hall sensors, while from 1985-9 industrial pull joined scientific push and a prototype EddyScan system for crack detection in aircraft was developed. The scientific focus then moved to transient eddy currents in the 1990s [3], as further research was undertaken, first on the technique and then (1995-2000) on applications as industrial pull increased. Activity switched to a product and the TRECSCAN system was developed from 2000-3, addressing aircraft inspection needs in the defence and aerospace sectors. Like ACFM and PEC, the development of transient eddy currents was heavily dependent upon background research into electromagnetic induction and eddy currents in particular. Here the early work benefited from collaboration between a government laboratory and a university. There was a requirement to deliver useful research outputs to the MoD customer in the early days of this development, but industrial pull appears to have strengthened progressively. This is consistent with the growing market for methods to prolong the life ageing aircraft. The first three examples build on related research into eddy currents. Apart from isolated pieces of pioneering research in various countries, the next example is of a technology developed from first principles, and it is therefore not surprising that it is still some way from acceptance, even though about 20 years have passed. In 1982-9 some fundamental scientific studies of magnetic methods for materials and stress characterisation were undertaken at Oxford University and Harwell Laboratory [4]. This led on to a programme of research into NDE stress measurement, 1989-93, with progressively stronger industrial pull and support from the oil and gas industry; this led to trial applications of what became known as MAPS in 1993-5. The early applications demonstrated the need for further research into the technique as well as its application (1995-00). It was found necessary to implement further refinements to the underpinning physical model as well as to the MAPS instrument (2000-7), while at the same time beginning to commercialise the technology for niche applications in the oil and gas and rail sectors. The early stages of the development showed the importance of collaboration between university, RTO and end-user industry. Industrial pull waned in the middle period of the development and this, coupled with privatisation and successive company reorganisations, may have delayed the innovation process. The final example is of an important ultrasonic innovation, time-of-flight diffraction (TOFD), rather than another electromagnetic technique. Maurice Silk started research into TOFD [5] at the NDT Centre, Harwell Laboratory (UKAEA) in 1974 using ideas from previous research into neutron time-of-flight spectrometry. During the ensuing years (1974-82) the work was mainly laboratory research (scientific push). Other scientists became involved and the theory of ultrasonic diffraction was developed in 1981-83. The first major industrial application was to UKAEA’s Winfrith Reactor 1982-4. Soon afterwards (1983-4) TOFD used by UKAEA for their nuclear defect detection trials. Almost simultaneously (1984-90) there was further industrial pull when TOFD was developed for offshore and undersea use as an early activity of Harwell’s HOIS project. The first commercialisation came 1982-4 when Zipscan was developed and licensed. Soon afterwards in 1984, TOFD started to be used for major industrial inspections, especially nuclear pressure vessels and offshore structures. The first TOFD standard was published in 1993 and TOFD was soon accepted as a mainstream NDE method across industry. TOFD took about 20 years to move from initial research idea through to an industry standard. It is salutary to wonder how long exploitation would have taken had it not been for strong industrial pull in the mid-1980s from two separate energy sectors. TOFD had little input from the university research base in its early days, reflecting the strength of public sector
C.B. Scruby / NDE Research Makes a Difference
15
laboratories then, a different situation from the 21st century. Throughout the central period of development there was strong collaboration between researchers, developers and end-users, helped by national imperatives in the nuclear case and a well-established and effective joint industry collaborative project (HOIS) in the other. Another important element was the utilisation of ideas and technology from other fields. A common theme in all of these and similar developments has been the need to develop physical models of the technique under investigation. In many cases using models to perform predictive or interpretive calculations was a major exercise, with more limited computing facilities prior to the 1990s. A model was vital to understand the amplitude variations in TOFD data, as it has been for example to interpret the electrical signals from ACFM, TRECSCAN and PEC techniques. In the case of MAPS, modelling the effects of stress on magnetic parameters from first principles involves very difficult physics as well as computational power. However difficult or timeconsuming, robust physical models are, in the author’s view, vital for any new technology. They are needed, not only to interpret the data and design the best way to use it, but also to give credibility within the scientific and engineering communities.
3. Lessons to be learnt From the author’s experience and knowledge, there are a number of barriers to or brakes that slow down effective NDE research, i.e. research whose results make a positive difference to industrial practice. Two important hurdles are, on the one hand lack of understanding by researchers of industrial needs and culture, and on the other hand lack of understanding by industry of scientific issues and research culture. Research itself, or the development process that follows can be hindered by the wrong level of funding, more commonly too little but occasionally too much at a time when the team is unable to deliver what is anticipated. This leads on to the importance of correctly managing expectations. Often researchers are over-optimistic about what they will achieve and their speed of progress in order to secure funds. When they fail to meet their customer’s expectations the development may be dropped for the wrong reasons. Intellectual property (IP) can cause problems. Sponsors of research may insist on IP rights that are too restrictive and stifle creativity, while loose IP arrangements can dissuade companies from investing in technology. As already stated, a serious issue concerns gaps in the supply chain, i.e. between researchers, developers and end-users. In terms of TRLs, the problems usually arise when progressing from level 4 to level 7. Especially during the past 10 years, members of the NDE supply chain have undergone reorganisations, changes of status, mission and objectives. Staff have been lost, working relationships destroyed and the supply chain disrupted. Finally, human factors always play a part, the biggest hurdles being lack of trust and poor communication for whatever reason. The Engineering Doctorate in NDE is a very encouraging recent development, already proving its worth in terms of technology transfer from research to application. Accountable to both university and company, the student (research engineer) begins to bridge that TRL gap. What lessons can be learnt of the ingredients for successful NDE research? The following list is not exhaustive, nor is every ingredient always necessary: 1. Adequate resources - people, facilities, environment, timely funding 2. Scientific excellence - creativity and lateral thinking balanced against penetration and focus; correct fundamentals essential for robust application
16
C.B. Scruby / NDE Research Makes a Difference
3. 4. 5. 6. 7. 8. 9. 10. 11. 12.
Technology push balanced against industry pull throughout Interdisciplinary collaboration, networking and international links Import of ideas, results & technology from other fields Industrial pull founded on sound business needs or regulatory imperatives Supportive organisational structures with long-term vision Viable exploitation route along “joined up” technology supply chain Committed individuals to champion and drive innovation process Trust, good communication and shared objectives within the whole “team” Proprietary secrecy balanced against publication and scientific credibility Good timing, grasp of opportunity, achievable timescales
The author is tempted to add: serendipity, since chance events often seem to unlock research and stimulate vital creative leaps; patience, since it is difficult to predict what research will produce and when.
4. Concluding Remarks Before discussing strategy for successful research in NDE, it is important to capture the present trends in the field of NDE. Encouragingly, most recent market surveys have predicted a steady growth in use of NDE by industry. This is driven ultimately by the needs of society for greater assurance of the safety of engineering structures. Linked with this is a heightened awareness of the need for environmental protection. New materials & new designs are being used that require new inspection technology. There is also a move towards greater automation, and the willingness to invest in high technology solutions to reduce inspection costs, improve quality, speed up inspection and sentencing. In some cases the move is towards reducing the need for inspections that interrupt service by new strategies such as structural health monitoring (SHM).
Mathematics Materials characterisation
Physics
Manufacturing & product quality Techniques
Technology & science transfer Mechanical engineering Materials science
NDE Research Applications
Supply chain
Electronic engineering
In-service structural integrity & assessment
Condition & health monitoring
Other disciplines Figure 4. NDE research and linked engineering disciplines
C.B. Scruby / NDE Research Makes a Difference
17
As a long-term strategy there is a desire to integrate NDE more strongly into the engineering life cycle, so that the benefits of NDE are weighed against reductions in the whole life cost of an asset. To do so requires the development of linkages with material science, engineering design, structural integrity and assessment. NDE sits at the centre of a complex network of engineering disciplines as Figure 4 shows; these needs to be understood and exploited. Recent years have seen large changes not only in the large users of NDE technology, but also in the supply chain. Equipment supply and inspection service companies have changed hands, merged and in some cases been bought by large companies. Such changes are likely to continue in the future. Without any doubt the NDE industry will continue to encounter technical challenges that can only be solved by consistent, high quality research. What are likely to be the main elements of a future NDE research strategy? The following list indicates some of the likely priorities: 1. Modelling, always essential for scientific understanding and to give confidence in product quality and for safety-critical applications 2. Improved quantification of results, characterisation and discrimination 3. More advanced data analysis, imaging and visualisation 4. Greater understanding of and improvement to reliability 5. Raising inspection speeds and reducing human factors through automation and autonomous systems 6. Incorporation of technological advances from other fields 7. Addressing new materials, designs, difficult applications & environments 8. Earlier detection of materials & structural degradation & failure 9. Technologies and strategies to facilitate reliable SHM This is a very full and challenging list. It can only be achieved through greater collaboration & integration with other disciplines & fields. It also requires the long term education and training of high calibre engineers for all stages of the research and innovation process. The UK Research Centre in NDE is a university-industry partnership that was established nearly 5 years ago to harness the UK’s research base to meet these longterm challenges, building on and learning from past experience, and hopefully avoiding some of the pitfalls. Its vision is to make a lasting difference to NDE technology through well-planned world-class research, and to invigorate the NDE profession through the provision of highly trained engineers. To conclude, NDE research does make a difference. It is impossible to respond to the challenges of tighter regulation, new materials and applications, new products and plant, more stringent operational conditions, longer life, higher accuracy, reliability, long terms global trends, changes in industry, rising public expectation of safe and environmentally secure operation, and the commercial drivers of faster, better, cheaper products without research.
References [1] [2] [3] [4] [5]
W.D.Dover, R.Collins and D.H.Michael, Phil. Trans. R. Soc. Lond. A320, (1986) 271-283. P.Crouzen, Proceedings of 9th European Conference on NDT, Berlin, (2006) in press S.K.Burke, G.R.Hugo and D.J.Harrison, Review of Progress in Quantitative Non-Destructive Evaluation, 17A, (1998) 307-314 D.J.Buttle, C.B.Scruby, J.P.Jakubovics and G.A.D.Briggs, Proc Roy Soc Lond. A414, (1987) 469 497. M.G.Silk and B.H.Lidington, Harwell Report, AERE-R7774 (1974).
18
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-18
Industrial Applications of 3MA – Micromagnetic Multiparameter Microstructure and Stress Analysis Gerd DOBMANN1, Iris ALTPETER1, Bernd WOLTER1, Rolf KERN1 1 Fraunhofer IZFP, Germany
Abstract. Micromagnetic NDT techniques like the measurement of the magnetic Barkhausen noise, the incremental permeability and the harmonic analysis of the tangential magnetic field allow deriving inspection procedures to online monitoring and control machinery parts and components in production processes in order to characterize mechanical properties like hardness, hardening depth, yield and tensile strength. These types of inspection procedures continuously were further developed in the last two decades so that today the second generation of system hard and software is in industrial use. The application is in steel industry where steel sheets in hot-dip-galvanizing lines were annealed after cold rolling but also in heavy plate rolling mills where after thermo-mechanical rolling special textures and texture gradients can occur. An increasing number of applications are also to find in the machinery building industry and here especially in case of machinery parts of the car supplying industry. Besides mechanical hardness determination the measurement of residual stresses and the detection of inhomogeneities in the surface of machined parts is an inspection task. In different case studies the advantage to implement a micromagnetic NDE technique into the industrial processes is discussed. Keywords. Micromagnetic NDE, hardness, hardening depth, residual stresses, yield strength, steel industry, steel sheets, heavy plates, machinery building, automotive
Introduction The reason to develop 3MA (Micromagnetic-, Multiparameter-, Microstructure-, and stress-Analysis), starting in the late seventies in the German nuclear safety program, was to find microstructure sensitive NDT techniques to characterize the quality of heat treatments, for instance the stress relieve of a weld. George Matzkanin [1] just had published a NTIC report in the USA to the magnetic Barkhausen noise. The technique was sensitive to microstructure changes as well as to load-induced and residual stresses. Therefore a second direction of research started in programs of the European steel industry and the objective was to determine residual stresses in big forgings. Beside the magnetic Barkhausen effect also a magneto-acoustic-one became popular [2]. The technique has based on acoustic emission measurements during a hysteresis cycle and was – because of the high amplification – also sensitive to electric interference noise. Therefore the acoustic Barkhausen noise technique has never found a real industrial
G. Dobmann et al. / Industrial Applications of 3MA
19
application. Later further micromagnetic techniques were developed: the incremental permeability measurement, the harmonic analysis of the magnetic tangential field and the measurement of the so-called dynamic or incremental magnetostriction by use of an EMAT [3, 4]. The methodology of the Micromagnetic-, Multiparameter-, Microstructure-, and stress- Analysis (3MA) in detail is described in [4]. On the basis of a multiple regression model, describing target quantities like hardness or yield strength as a function of measured micromagnetic quantities, the unknown model parameters are determined in a calibration step. By using a least squares approach the unknown parameters are the solution of a system of linear equations. 3MA only can be applied at ferromagnetic materials. Here the techniques are especially sensitive to mechanical property determination as the relevant microstructure is governing the material behavior under mechanical loads (strength and toughness) in a similar way as the magnetic behavior under magnetic loads, i.e. during the magnetization in a hysteresis loop. Because of the complexity of microstructures and the superimposed stress sensitivity there was a need to develop the multiple parameter approach. Whereas the first generation of 3MA equipments was basing on the magnetic Barkhausen noise and magnetic tangential field analysis only, 3MA equipment exist now in the forth generation also integrating incremental permeability and eddy current impedance measurements (see Figure 1). More than 100 installations are in use in different industrial areas. This mainly covers the steel and machinery building industries.
Figure 1. TCP-IP-based 3MA equipment and software in combination with a laptop
1. Applications in the steel industry 1.1 Steel Strip Inspection A lot of experiences with 3MA in the last 2 decades were to the continuous mechanical property determination at steel strips, designed to produce car bodies [5, 6], running with a speed of 300m/minute for instance in a continuous galvanizing and annealing line. Yield strength (Rp0.2), tensile strength (Rm), planar and vertical anisotropy parameters (rm, 'r) are in the focus of quality assurance measures [4], all of them are defined by destructive test and cannot be measured continuously. Therefore 3MA correlations were calibrated. Figure 2 shows a yield strength profile along a coil of 2.5 km length [5]. At the beginning and the end an unacceptable increasing of strength is detected higher than
20
G. Dobmann et al. / Industrial Applications of 3MA
the upper acceptance level (blue line). The strength values are calculated by the 3MA approach from measured micromagnetic data. The red dots indicate the selection of specimens taken to destructive verification tests after performing NDT. The residual standard errors found by validation are in the range 4-7 % concerning the yield strength. Figure 3 shows a 3MA installation in the line of a strip producer; a robot is used to handle the transducer.
Figure 2. 3MA predicted Yield strength [5]
Figure 3. 3MA probe with robot at a strip line
1.2 Heavy plate Inspection
1600
1600
Elastic limit R p0.2 [MPa] (3MA)
Tensile strength R m [MPa] (3MA)
Ongoing research is to heavy plate inspection. The steel producer asks for the measurement of geometrical and mechanical properties, which have to be uniform along the product length and width, especially in the case of high-value grades used in off-shore application. Destructive tensile and toughness tests are performed by highly qualified and certified personnel according to codes and delivery conditions. The tests cannot be integrated into online closed loop control with direct feedback. To reliably test the mechanical hardness the surface must be carefully prepared by removing scale and decarburized surface layers and residual stresses are to relieve. The extraction of the test pieces and testing is very time and cost extensive. Costs in the range of several thousands Euro per year arise in a middle-sized heavy plate plant only by destruction of the test pieces. 1400 1200 1000 800 600 400 200 0
1400 1200 1000 800 600 400 200 0
0
200
400
600
800 1000 1200 1400 1600
Tensile strength R m [MPa] (destructive)
Figure 4. Tensile strength predicted by 3MA [6]
0
200
400
600
800 1000 1200 1400 1600
Elastic limit or yield strength Rp0.2 or R EH [MPa] (destructive)
Figure 5. Yield strength predicted by 3MA [6]
G. Dobmann et al. / Industrial Applications of 3MA
21
In case of a mother plate of several meters length the edges are usually subjected to other cooling conditions than the rest. Indeed, especially the plate ends are known to cool faster, generating an undesired increase in tensile strength Rm and yield strength Rp0.2. State-of-the-art is to cut-off the plate edges with non-conform properties based on empirical values concerning the cut-off length. As the destructive tensile test follows directly after the cut-off process of the edges, only the result of these tests can reveal the selection of a not appropriate cut-off length. This results in high costs due to reworking, pseudo-scrap and delayed shipment release; the European steel producers estimate their annual costs in the range of 11 million Euros. Knowing exactly the contour of the zone with unacceptable material properties would allow an open loop control of the cut-off process. Therefore heavy plate producers will replace the destructive quality inspection of test pieces by a NDT technology [6] applying 3MA (see Figure 4 and 5). By a manufacturer-specific calibration residual standard errors of 10 MPa (Rm), 20 MPa (Rp0.2), and 4HB in the Brinell hardness can be obtained. It should mention here that in the 3MA calibration also other measuring quantities can be integrated so far they provide other independent information, for instance elastic properties. By using ultrasonic waves propagating in thickness direction, i.e. a compressive wave excited by a piezoelectric transducer (index L) and two linearly polarized shear waves (polarized in, index SHR, and transverse, index SHT, to the rolling direction) excited by a EMAT, normalized time-of-flight quantities can be derived describing crystallographic texture effects. Taking into account these quantities (tSHR/tL, tSHT/tL, (tSHR-tSHT)/tL) together with the micromagnetic parameters then a regression result is obtained again reducing the residual standard error.
2. Application in Automotive and Machinery Building Industry 2.1 Car Engine casting To reduce the weight of the power supply unit the car combustion engines cylinder crankcases can be made of cast iron with vermicular graphite (GJV), because this material in a Diesel engine allows a higher loading pressure even by reduced wall thickness. However, the service live of machining tools is during processing an engine block made from GJV substantially smaller compared with a block from cast iron with lamellar (flake) graphite (GJL). work on - relevant range
lamellar graphite
GJL
transition zone
vermicular graphite
GJV
Figure 6. Microstructure gradient obtained in a cylinder region of a cast engine [7]
This disadvantage can be eliminated by an innovative casting technology that produces a continuous microstructure gradient in the cast iron from lamellar graphite at
22
G. Dobmann et al. / Industrial Applications of 3MA
the inner surface of the cylinders to vermicular graphite in radial direction. By implementing some chemical additives into the core of the mould which can diffuse in the cast iron during the solidification process in the mould the gradient with a continuous transition from lamellar graphite and finally vermicular graphite is obtained. However, the technology can only be used by the casters so far the gradient quality can be characterized and monitored by NDT. Figure 6 documents in a micrograph such a gradient beginning at the left side with cast iron (inner cylinder surface) and lamellar graphite followed by a transition region and vermicular graphite on the right side. 3MA techniques always cover a certain analysing depth depending on the magnetising frequency and geometrical parameters of the magnetisation yoke, etc. So far the gradient has different graphite compositions within the analysing depth, 3MA quantities should be influenced. Based on measurements at an especially designed calibration test specimen set 3MA quantities were selected to image the gradient with optimal contrast. As reference quantity to calibrate 3MA the local thickness of the GJV-layer was evaluated by using micrographs and optimized pattern recognition algorithms in the microscope. A special designed transducer head was developed to scan the cylinder surface by line scans in hoop direction and rotating the head, then shifting the head in axial direction to perform the next line scan. Figure 7 and Figure 8 show as example the coercivity images derived from the tangential field strength evaluation[3] (HC0 in A/cm) and line scans covering an angle range of 190°.
Figure 7. Coercivity image of a reference block made from GJV
Figure 8. Coercivity image of block with GJV/GJL gradient
Combining different 3MA quantities in a multiple regression the thickness of the GJL layer was predicted. A regression coefficient of R2= 0.93 and a residual standard error of V = 0.06 mm was obtained [7]. 2.2 Wheel Bearing Inspection The fixation of the inner ring of wheel bearings is performed by a wobble riveting process. As a consequence a residual stress is built up in the ring which may not exceed a limit value of about 300 MPa to get a perfect quality. The usual technique to inspect the residual stress state is x-ray diffraction which is destructive in nature because it requires a preparation of the test location. Furthermore it can only be performed statistically. The 3MA technique allows a fast non-destructive estimation of the residual stress level (Figures 9, 10). After a calibration step by using x-ray reference values a 100% quality inspection of these parts is possible. The calibration procedure requires a coincidence of the 3MA and x-ray calibration positions
23
G. Dobmann et al. / Industrial Applications of 3MA
because residual stress varies along the circumference. That means the 3MA data have to be recorded in a first step before the x-ray test location is prepared by etching. According to Figure 10 the residual standard error in the calibration is in the 20 MPa range. Besides the residual stress additionally the surface hardness can be measured. 250
Analysing Depth: 100 μm
Residual Stress [MPa] (X-ray)
200
150
100
50
0
Adj.R² = 0.941 1 = 19.0 MPa
-50 -50
0
50
100
150
200
250
Residual Stress [MPa] (3MA)
Figure 9. 3MA-Probe at test location
Figure 10. Residual stress calibration
2.3 Evaluation of Microstructure and Stress Gradients Machined parts in most of the cases have more or less steep gradients in their properties near the surfaces. To improve the lifetime of mechanical highly stressed machinery components the bearing areas are surface-hardened from the μm- up to the millimetre range depending on the requirements and on the hardening technology. 80 70
3MA / Nht 700 [μm]
Adj R² = 0,8211
60 50 40
Adj R² = 0,9151
30 20
3MA Value
10
Nht700 Value
0 0
10
20
30
40
50
60
70
Optical Result [μm]
Fig.11. Comparison of nitrating hardening depth measured by 3MA and Nht 700 (Vickers) versus optical result
Additional surface finishing by grinding can superimpose surface near defects of microstructure and residual stresses which can result in a part breakdown. To inspect the production quality in many cases not only the properties immediately at the surface but also information of the properties below the surface are desired. 3MA is an effective tool to investigate the properties near the surface as well as the range below the surface up to several millimetres in depth. One example of a 3MA application in industry is the determination of nitrating hardening depth NHD of piston rings on the flank side and on the tread surface. Typical values of nitrating hardening depth are between 60 and about 100 μm. It is found by the user that the reproducibility of the non-destructive values of hardness and hardening depth in piston rings is better than the conventional testing by a
24
G. Dobmann et al. / Industrial Applications of 3MA
metallographic Vickers hardness test (Nht700), as can be seen in Figure 11 [8]. The reason of that behaviour seems to be the difference in the lateral resolution of the conventional and the non-destructive testing method. Due to a diameter of the 3MA receiver coil of about 2 mm the 3MA values are covering a much larger inspection area. Fast data evaluation by 3MA allows a complete production feedback control. The occurrence of grinding defects, e. g. in gear wheels, is a main problem since many years which is caused by too much heat input during the grinding process. Modern grinding tools allow much higher grinding speed compared to former machines but on the other side this can result in more defects. To get information on the quality of grinded microstructure states the common method in industry is the nital etching technique. Grinding defects are indicated by the discoloration of the surface. This technique is effective as long as the surface information is sufficient to estimate the quality. But it fails if in a preceding production step defects are produced below the surface which are covered in the next production step by a perfect finishing. Several examples of defective gear wheels investigated by hole drilling method and x-ray diffraction have shown that in a depth of 100 μm high tensile stresses up to several 100 MPa can be present whereas at the surface a perfect compressive state of several hundred MPA has been found. These hidden defects cannot be detected by nital etching. As a consequence after some time small cracks are covering the surface due to stressrelieve even without a mechanical load.
Figure 12. Hardness calibration at various depths; hardness values determined by 3MA versus target values
Figure 13. Residual Stress calibration at various depths; RS values determined by 3MA versus X-ray reference values
Since several years IZFP has gained experience in the non-destructive detection and quantitative evaluation of such grinding defect gradients by 3MA in cooperation with industrial partners and in different research and development projects [9, 10]. After a calibration step 3MA can be used to evaluate different target values simultaneously, especially the hardness and the residual stress at the surface and in several depths below the surface (Figures 12 and 13). To get unambiguous results calibration must be done carefully. Calibration is mainly determined by well defined calibration specimens and only valid to the target ranges available by calibration. In most cases calibration is restricted e. g. to the material, to the actual machining parameters and even to the 3MA probe in use. If any variation occurs, its influence on the validation of the existing calibration has to be checked and if necessary a recalibration or extension of the existing calibration has to be performed to include any disturbances. These limitations and the calibration effort may be seen as a disadvantage of 3MA. But if an optimal calibration is developed the fast non-destructive
G. Dobmann et al. / Industrial Applications of 3MA
25
determination of various quality parameters which is desired concerning expensive security related parts justifies this effort.
3. Conclusion 3MA is a matured technology and a wide field of applications is given. However, besides the success story we also can find critical remarks from industrial users. These are mainly to the calibration efforts and problems of recalibration if a sensor has to be changed because of damage by wear. Therefore actual emphasis of R&D is to generalize calibration procedures.
4. Acknowledgements The authors very much appreciate to acknowledge the contribution to the result by companies as ThyssenKrupp Stahl AG, Duisburg, ArcelorMittal Research, Metz, Dillinger Hütte GTS AG, Dillingen, Halberg Guss GmbH, Saarbrücken, and Schaeffler KG, Schweinfurt.
References [1]
G.A. Matzkanin, et al., The Barkhausen Effekt and its Application to Nondestructive Evaluation, NTIAC report 79-2 (1979) (Nondestructive Testing Information Analysis Center, San Antonio, Texas) 1-49. [2] W.A. Theiner, E. Waschkies, Method for the non-destructive determination of material states by use of the Barkhausen-effect (in German), Patent DE 2837733C2 (1984). [3] G. Dobmann et al, Barkhausen Noise Measurements and related Measurements in Ferromagnetic Materials; in Volume 1: Topics on Non-destructive Evaluation series (B.B. Djordjevic, H. Dos Reis, editors), Sensing for Materials Characterization, Processing, and Manufacturing (G. Birnbaum, B. Auld , Volume 1 technical editors), The American Society for Non-destructive Testing (1998) ISBN 1-57117067-7. [4] I. Altpeter, et al., Electromagnetic and Micro-Magnetic Non-Destructive Characterization (NDC) for Material Mechanical Property Determination and Prediction in Steel Industry and in Lifetime Extension Strategies of NPP Steel Components, Inverse Problems 18 (2002) 1907-1921. [5] M. Borsutzki, Process-integrated determination of the yield strength and the deep drawability properties rm and 'r on cold-rolled and hot-dip-galvanized steel sheets (in German); Ph.D. thesis, Saar University, Saarbrücken, Germany, 1997. [6] B.Wolter, G. Dobmann, Micromagnetic Testing for Rolled Steel, European Conference on Nondestructive Testing (9) (2006) Th. 3.7.1, 25.-29. 09. 2006, Berlin. [7] M. Abuhamad, I. Altpeter, G. Dobmann, M. Kopp, Non-destructive characterization of cast iron gradient combustion engine cylinder crankcase by electromagnetic techniques (in German), DGZfPAnnual Assembly (2007), Fürth (to be published). [8] IZFP Annual Report, (2004), Saarbrücken, Germany. [9] W. A. Theiner et al., Process Integrated Nondestructive Testing For Evaluation Of Hardness; in the proceedings of the 14th World Conference on Nondestructive Testing (14th WCNDT), (1996) 573, New Delhi, India. [10] B. Wolter et al., Detection and Quantification of Grinding Damage by Using EC and 3MA Techniques, in the proceedings of the 4th International Conference on Barkhausen Noise and Micromagnetic Testing, 03-04 July 2003, Brecia, Italy, 159-170.
26
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-26
3D Nonlinear Finite Element Analysis of Electromagnetic Inspection of Defects in Steel N.Takahashi 1 and Y.Gotoh 2 Abstract. The electromagnetic inspection technology is commonly used to evaluate defects in steel in various power generation plants because of its ability to detect quickly. In this paper, the electromagnetic inspection methods using an ac magnetic field, or a biased ac field are proposed. The behavior of the flux in steel is examined using 3-D FEM that takes into account the initial magnetization curve, hysteresis (minor loop) and eddy currents in order to improve the inspection method. Keywords. Electromagnetic inspection, 3-D nonlinear FEM, hysteresis, magnetization curve, opposite side defect in steel
1. Introduction The electromagnetic inspection method offers the possibility of quick detection of various kinds of defects, such as the outer side defects and plural cracks [1]. Since the permeability of the steel is usually not uniform, the electromagnetic inspection of steel has a magnetic noise. Therefore, a strong magnetic field is used for the inspection of defects in a ferromagnetic material, such as a steel wall of the oil tank or the steel tube etc. [2]. The non-uniformity of permeability in steel is reduced when a magnetic field is increased. Therefore, the ac or dc strong magnetic field is used for the inspection method using dc field and eddy current testing or the magnetic flux leakage testing (MFL) etc. [3,4]. In order to improve these inspection methods, the detailed analysis of 3-D flux and eddy current distribution should be performed. However, a detailed examination of the behavior of flux distribution etc. under the electromagnetic inspection using a strong magnetic field is difficult, because the magnetic property of steel is nonlinear and eddy currents are induced. Although there has been a lot of research in defect detection analysis [5-7], little work has been done in the 3-D analysis when the material is magnetic. In this paper, problems of 3-D finite element analysis in electromagnetic inspection, such as the inclusion of minor loops for the detection under ac and dc excitation, are discussed. The electromagnetic inspection method using a dc magnetic field and a minute alternating magnetic field has been proposed [8]. The behavior of flux in steel is examined using a 3-D finite element method that takes into account hysteresis (minor loop) and eddy currents. It is shown that the detection of a defect is possible by the differential permeability of the minor loop as its position in the BH plane is affected by 1 Norio Takahashi is with Department of Electrical and Electronic Engineering, Graduate School of Natural Science & Technology, Okayama University, 3-1-1 Tsushima, Okayma 700-8530, Japan. (telephone: +8186-251-8115, fax: +81-86-251-8258, e-mail:
[email protected]. jp). 2 Yuji Gotoh is with Department of Mechanical and Energy Systems Engineering, Faculty of Engineering, Oita University, 700 Dannoharu, Oita, 870-1192, Japan. (telephone: +81-97-554-7795, fax: +81-97-554-7790, e-mail:
[email protected]).
N. Takahashi and Y. Gotoh / 3D Nonlinear Finite Element Analysis of Electromagnetic Inspection
27
the existence of the defect. The flux and eddy current distribution in steel, having plural cracks, are analyzed and it is shown that the detection of plural cracks, when the distance between them is very short, is possible using the differential type two search coils which is set parallel to the steel plate [9]. Steel tubes are used in the heat exchanger in petrochemical plants. Since these steel tubes are grouped in a bundle, it is necessary to inspect the existence of defects from the inside of each tube. Therefore, the possibility of detection of outer side defects in steel tubes using an inner coil in the alternating flux leakage test is examined by analyzing the detailed behavior of flux and eddy current distribution [10]. 2. Evaluation of Detection Method of Opposite Side Defect using DC Field and Minute AC Field Taking Account of Minor Loop 2.1 Model and Method of Analysis Figure 1 shows the model of 1/2 the domain needed to analyze the detection of the opposite side defect in a steel plate. This model is composed of the yokes for dc and a minute ac magnetic field and a search coil. The dc exciting current is 3A and the minute ac exciting current is 0.5A (1kHz). The flux density B in the steel is produced by the dc magnetic field and the minute ac magnetic field. The magnetic field is analyzed using 3-D edge-based hexahedral nonlinear FEM and the step-by-step method taking account of hysteresis (minor loop) and eddy currents in the steel plate. The basic equation of eddy current analysis using the A-Imethod is given by: · § wA Jo V ¨ gradI ¸ ¹ © wt § wA ·½ div ® V ¨ gradI ¸¾ 0 ¹¿ ¯ © wt
rot (QrotA)
(1) (2)
where A is the magnetic vector potential, I is the scalar potential, v is the reluctivity, Jo is the current density and V is the conductivity. The minor loop is modeled using these upper hysteresis curves (SS400) [1]. It is assumed that the obtained B and H are at the point b (Hmin, Bmin) on the upper loop as shown in Figure 2. If the calculated flux density Bc at the Newton-Raphson (N-R) iteration is larger than Bmin, then Bc should be located at the point d (Hd, Bc) on the lower minor loop. Hd on the lower minor loop is given by the following equation, if the upper loop is symmetrical with respect to the middle point e: Hd
H g 2H e H g .
(3)
2.2 Behavior of Minor Loop and Inspection of Opposite Side Defect Figure 3 shows the calculated result of a minor loop at a surface point in the steel with and without an opposite side defect. The figure indicates that the dc flux density near the defect in steel is increased when there exists an opposite side defect and a minor loop is generated at the high flux density on an initial magnetization curve. The figure shows that the differential permeability of the minor loop becomes small, when there exists an opposite side defect in the steel. Figure 4 shows the distribution of the differential relative permeability Pd on a minor loop with and without an opposite side defect. Figure 4 (a) shows that the differential relative permeability is increased near the surface of the steel plate when there are no
28
N. Takahashi and Y. Gotoh / 3D Nonlinear Finite Element Analysis of Electromagnetic Inspection
22
52.5
.5
.5 16 20
19
dc-yoke dc-exciting coil (3A)
B
2
initial magnetization curve upper minor curve
29
33
steel plate (SS400)
3.35
1.35 7.65
lift-off=0.1 3
x
f (Hf, Bf)
=
=
150 ac-exciting coil (1kHz, 0.5A)
g (Hg, Bg)
=
z y
a (Hmax, Bmax) 2.7 9 1.4 4 ac-yoke search coil 10.18 0.56
4.28
4.7
10 5
=
c (Hc, Bc)
2.95
e (He, Be) d (Hd, B䌣)
Dd=1
opposite side defect
b (Hmin, Bmin) Dw
lower minor curve
0
H
Dw=0.5
Figure1. Inspection model of steel plate with outer side defect (1/2 domain). 2
Figure 2. Explanation of minor loop. ac-yoke
search coil (40turns) differential Pd
1.6
1200
B (T)
with an opposite side defect
1000
1.2
800
without an opposite side defect
600
0.8
400
z
initial B-H curve
200
0.4 0
0
x
0
2000
4000 6000 H (A/m)
8000
steel plate (SS400)
(a) without an opposite side defect
differential Pd 1200
Figure 3. Effect of opposite side defect on minor loop (calculated).
1000 800 600 400 200 0
opposite side defect
(b) with an opposite side defect Figure 4. Distribution of the differential relative permeability Pd on a minor loop in the steel plate with and without an opposite side defect (dc=3A, ac=1kHz, 0.5A).
defects. However, the permeability between the opposite side defect and the surface of the steel is reduced as shown in Figure 4 (b). Since the dc flux is distributed near the surface of the steel plate, the minute ac flux density dose not penetrate as far as the opposite side defect. During the inspection, the dc and ac yokes are moved along the x-direction by 1mm pitch, keeping the lift-off at 0.1mm. Figure 5 shows the measured inspection result of the change of ac flux density 'B detected by the search coil due to the outer side defect. 'B is defined by 'B=|B| (at defect position)-|B| (at no defect position, x=10mm)
(4)
29
N. Takahashi and Y. Gotoh / 3D Nonlinear Finite Element Analysis of Electromagnetic Inspection
'B in the search coil is calculated by 3-D non-linear FEM taking account of hysteresis (minor loop) and eddy current. After 35 steps (about 2 periods), almost steady state result can be obtained. The figure shows that the measured and calculated peak values of 'B are almost in good agreement. Moreover, 'B is decreased near the position of the opposite side defect. This is due to the fact that the dc flux density near the position of the opposite side defect in steel plate is increased and as a result, the permeability of the steel is decreased. The figure suggests that it is possible to detect the opposite side defect in a steel plate by using the proposed inspection method. measured
0
'B (x10-4T)
calculated -20
-40
Dd=1
-60 -10 -7.5 -5 -2.5
0
2.5
5 7.5 10 position x (mm) opposite side defect
Dw=0.5
Figure 5. Change of flux density 'B when there exists an opposite side defect (dc=3A, ac=1kHz, 0.5A).
3. Alternating Magnetic Flux Leakage Testing for Detection of Plural Cracks 3.1 Inspection Method and Modeling Figure 6 (a) shows a model of the alternating magnetic flux leakage test that detects plural cracks. The amplitude of the current is 1A(rms). The gap between the leg of the yoke and the surface of the steel is 0.2mm. Figure 6 (b) shows the proposed differential type search coils for detecting the parallel component Bx of leakage flux from plural cracks. The leakage flux Bx which is uniformly distributed over the steel surface is measured using the search coil E. The local leakage flux Bx from the cracks is measured using the search coil D. The difference between Bx obtained by the search coil D and that by the search coil E is used for detecting the number and the size of plural cracks. The sizes of these coils were optimized using the evolution strategy. The search coils (thickness < 0.1mm) can be located under the legs of the yoke. The frequency is chosen as 1kHz, resulting in a skin depth of 0.15mm (the relative permeability is assumed to be 2500).
yoke Yoke
z
Plate
Distance L:0.5mm y
29
E
w=S
16.5
Sw -
3
52
2
29
Steel plate steel plate (SS400)
22 .5
19
2
52.552.5
19
56.5
exciting Exciting coilcoil
10 5
D
Bx search coil E
SlSl-E=59 =59
0.1
0.06
x
150
search coils Search coil y
z
Crack (Width Cw:: 0.01mm)
Depth Cd:1mm :1mm
Bx search coil D
Position of search coil D (D)
x
(a) bird’s eye view (1/2 region) (b) search coils for detecting plural cracks Figure 6. Model for alternating flux leakage testing of plural cracks.
30
N. Takahashi and Y. Gotoh / 3D Nonlinear Finite Element Analysis of Electromagnetic Inspection
Cd=1
Bx [x10-4 T]
100 80
Cd=0.5
60
Cd=0.1
40 20 0 -20 -1.5
No-crack -1
-0.5
0
L=0.5
Figure 7. Detection of Bx using differential search coil (Cw=0.01mm, Cd=1mm, L=0.5mm, 1kHz, 1A, calculated, with hysteresis).
0.5
1 1.5 Position [mm]
Crack position (Cw=0.01)
Figure 8. Effect of depth of cracks on Bx (1kHz, 1A, calculated, with hysteresis)
3-D FEM using the 1st order hexahedral edge element is applied. The flux and eddy current are analyzed by the step-by-step method taking account of the non-linearity of the steel plate. In order to obtain the steady state result, the calculation is carried out for 2.5 periods (=160 steps). The time interval Ǎt of the step-by-step method is chosen as 1.5625x10-5 sec. 3.2 Detection of Plural Cracks using Horizontal Coils The detection characteristics are analyzed by a nonlinear calculation using the hysteresis curves. Figure 7 shows the distribution of Bx of one, two and four cracks detected using the differential type coil. The figure illustrates that it is possible to evaluate plural cracks by using the amplitude of the parallel component Bx of leakage flux detected by the differential search coil. Figure 8 shows the effect of the depth of the cracks when there are two cracks. The figure shows that the amplitude of Bx is increased as the crack depth grows. 4. Electromagnetic Inspection Method of Outer Side Defects on Steel Tubes using an Inner Coil 4.1 Inspection Model and Conditions Figure 9 shows the inspection model of the outer side defect of a steel tube (SUS430). The proposed inner inspection probe is also shown in the figure. The inspection probe is composed of a yoke, an exciting coil and a search coil for detecting the perpendicular component |Bx| of leakage flux due to the outer side defect. The outer side defect is a circumferential one. The frequency is chosen as 60Hz (commercial frequency) resulting in a skin depth equal to 2.31mm (maximum relative permeability (=434) in the steel tube is used for the calculation of the skin depth). The exciting current is 5A(rms). The conditions of analysis and experiment are as shown in Table 1. 4.2 Outer Side Defect in a Steel Tube Figure 10 shows the distribution of calculated and measured |Bx| in a search coil. |Bx| is obtained by moving the inspection probe in the z-direction inside the steel tube at the
N. Takahashi and Y. Gotoh / 3D Nonlinear Finite Element Analysis of Electromagnetic Inspection
Table 1. Condition of analysis and experiment 202 turns, 60Hz, 5A (rms) 50 turns, Width (Sw)=3mm, Height (Sh)=1.65mm, Length (Sl)=2.56mm, Lift-off (Lo)=0.2mm SUS430, V=1.82x106 S/m, Diameter=25I, Thickness (t)=1.5mm, Pr-max=434 SS400, V=7.51x106 S/m, Maximum relative permeability Pr=3000 Width (Dw)=2mm, Depth (Dd) =0.5mm, Circumference defect 88095, 83232 N-R method: 1.0x10-3 T, ICCG method: 1.0x10-5
Exciting coil Search coil Steel tube Yoke Outer side defect Nodes and elements Convergence criterion
5
steel tube (SUS430, 25㱢) exciting coil (202turns)
70 60
-4
search coil (Bx)
Bx [x10
Sw=3
80 59.6
50turns
me asured 40 30 20
4.5 Sl=2
20.4
calculated
50 T]
10.5
31
.56 S
5 1.6 h=
yoke (SS400)
10 0 -10
-5
0
z t=1.5
y
x D w=2
Figure 9. Inspection model for outer side defect of steel tube (1/4 domain).
5
10 position z [ mm]
position of outer side defect
Figure 10. Inspection waveform of leakage flux (60Hz,5A).
lift-off of 0.2mm. The calculated result is in agreement with measurement. The figure illustrates that the outer side defect in the steel tube can be detected using the proposed inspection method. 4.3 Application to the Steel Tube with Aluminum Cooling Fin In a petrochemical plant, the steel tube is sometimes used with aluminum cooling fins. Therefore, the possibility of applying the proposed inspection method for detecting the outer side defects on a steel tube with cooling fin is examined. Figure 11 shows the inspection model of the steel tube (SUS430) with aluminum cooling fin. The outer side defect width (Dw), defect depth (Dd) and defect length (circumference direction, Dl) are 0.5mm, 0.5mm and 10mm, respectively. The nonlinear analysis was carried out. The non-uniformity of permeability and conductivity in steel is neglected. The conductivity V of the aluminum fin is 3.5x107 S/m. Figure 12 shows the eddy current distributions in the steel tube with and without fin. The figure shows that the eddy current density is maximum at the inner boundary of the fin with high conductivity. The maximum flux density |B|max in the steel tube with fin is 1.68T and |B|max without the fin is 1.51 T. The flux density in the steel tube is increased when the fin is put on the tube because of the opposing flux due to the eddy currents. Figure 13 shows the average flux density |Bx| in a search coil calculated along the zposition inside the steel tube with and without the fin. The results under the dc excitation are also shown. The figure shows that the leakage flux from the steel tube with the fin is larger than that without the fin under ac excitation. The leakage flux is increased due to the larger than that without the fin under an ac excitation. The leakage
32
N. Takahashi and Y. Gotoh / 3D Nonlinear Finite Element Analysis of Electromagnetic Inspection steel tube (SUS430, 25㱢)
1 .5
2.5
2 2
search coil (Bx)
tube fin
yoke fin of aluminum
exciting coil
exciting coil (202turns) yoke (SS400)
outer side defect Dw=0.5, Dd=0.5, Dl=10
z y
x
27.5
Figure11. Inspection model of the steel tube with the aluminum fin. eddy current [x105 A/m2] 14 12 10 8 6 outer side defect
4 2
z
0
x
steel tube (SUS430)
1.5 2.5
fin of aluminum
(a) without fin (b) with fin Figure 12. Distribution of eddy current density in steel tube with the aluminum fin (60Hz,5A, Dw=0.5mm, Dd=0.5mm). with fin (60Hz) 30
without fin (60Hz)
15
with fin
20 10
with fin and without fin (DC) : with fin : without fin
5
0 -8
-6
-4
-2
0
2
10
without fin
4 6 8 position z [mm]
position of the fin of aluminum position of outer side crack (Dw=0.5, Dd=0.5, Dl=10) 2
Bx [x10-4 T]
Bx [x10-4 T]
20
0 0
20
40
60 80 100 120 140 160 180 200 exciting frequency [Hz]
2
Figure 13. Effect of aluminum fin and alternating magnetization (5A, Cw=0.5mm, Cd=0.5mm, calculated).
Figure 14. Effect of exciting frequency (5A, calculated).
N. Takahashi and Y. Gotoh / 3D Nonlinear Finite Element Analysis of Electromagnetic Inspection
33
increased due to the eddy current in the steel tube and the fin. The ac excitation at 60Hz is appropriate from the viewpoint of the amplitude of the output signal as compared with the dc excitation. Figure 14 shows the maximum flux density in a search coil calculated by changing the exciting frequency in a model with and without fin when the exciting current is 5A (rms). As seen in the figure, the exciting frequency that is suitable for the inspection is around 20Hz – 60Hz. 5. Conclusions The results obtained are summarized as follows: (1) The principle of the inspection method of opposite side defects with ac and dc excitations is clarified by analyzing the magnetic property of the material. When the large dc magnetic field is impressed on a steel plate with the opposite side defect, the dc flux in steel bypasses the defect because of the magnetic saturation. As a result, the flux density between the opposite side defect and the surface of the steel is increased. The differential permeability of the minor loop due to the minute ac magnetic field is therefore decreased. This phenomenon can be used for the inspection of opposite side defects. (2) It is possible to evaluate plural cracks by using the amplitude of the parallel component Bx of the leakage flux detected by the differential search coil. (3) The alternating flux leakage test method using an inner coil at commercial frequency is able to detect the outer side defect in steel tubes with or without aluminum cooling fin. The ac excitation is more suitable than the dc excitation. References [1] Y.Sun, “An introduction to electromagnetic nondestructive testing”, Applied Electromagnetics and Mechanics, vol.13, pp.145-152 (1998). [2]N.Kasai㧘K.Sekine, and H.Maruyama, “Non-destructive evaluation method for far-side corrosion type flaws in oil storage tank bottom floors using the magnetic flux leakage technique", J. Jpn. Petrol. Inst., vol.46, no.2, pp.126-132 (2003). [3] H.Fujiwara, T.Sakamoto, T.Nishimine, and K.Kokubo, “Development of ac magnetic leakage flux testing system”, Proc. Int. Symp. Applied Electromagnetics and Mechanics, pp.527-528 (2001). [4] S.Nishino, “Development of magnetizing eddy current pipeline inspection tools”, The First US-Japan Symposium on Advances in NDT, pp.254-258 (1996). [5] G.Chen, T.Sugibayashi, M.Shiwa, and H.Yoneyama, “Investigation of subsurface flaw detectability of magnetic flux leakage testing”, Proc. Int. Symp. Applied Electromagnetics and Mechanics, pp.525-526 (2001). [6] K.Sekine, Y.Zhang, A.lizuka, and K.Nonaka, ”A Theoretical analysis of magnetic force acting on magnetic particles in the Immediate vicinity of surface flaws”, The First US-Japan Symposium on Advances in NDT, pp.396-401 (1996). [7] M.Katoh, K.Nishio, T.Yamaguchi, and S.Mukae, “FEM study on magnetic test of square bar by direct contact method”, Proc. FENDT ’94 and ROCSNT 9th Annu. Conf., pp.79-85 (1994). [8] Y.Gotoh and N.Takahashi, “Evaluation of detecting method with AC and DC excitations of opposite side defect in steel using 3D non-linear FEM taking account of minor loop ”, IEEE Trans. Magn., vol.44 (2008). [9] Y.Gotoh and N.Takahashi, “Detection of plural cracks in steel using horizontal coils – 3D FEM analysis considering hysteresis and non-uniformity of steel –”, IEEJ Trans. FM, vol.125, no.10, pp.835-840 (2005). [10] Y.Gotoh and N.Takahashi, “3D FEM analysis of electromagnetic inspection of outer side defects on steel tube using inner coil”, IEEE Trans. Magn., vol.43, no.4, pp.1733-1736 (2007).
This page intentionally left blank
Magnetic Materials
This page intentionally left blank
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-37
37
Evaluation of Irradiation Embrittlement in Fe-Cu-Ni-Mn Model Alloys by Measurements of Magnetic Minor Hysteresis Loops Satoru KOBAYASHI a,1 , Hiroaki KIKUCHI a , Seiki TAKAHASHI a , Katsuyuki ARA a and Yasuhiro KAMADA a a NDE and Science Research Center, Faculty of Engineering, Iwate University, 4-3-5 Ueda, Morioka 020-8551, Japan Abstract. Magnetic minor hysteresis loops of neutron-irradiated Fe-Cu-Ni-Mn model alloys varying Cu and Ni contents have been measured. For almost alloys minor-loop coefficients which are in proportion to internal stress decrease after neutron irradiation to a maximum fluence of 0.44 × 1019 n cm−2 . The decrease of the coefficients is strongly enhanced for alloys with high Cu and high Ni contents. Both magnetic and mechanical properties are correlated with each other and the coefficients are roughly in inverse proportion to yield strength. Keywords. Neutron irradiation, Magnetic minor hysteresis loops, precipitates
Introduction Neutron irradiation induces microstructural changes associated with an increase in a number density of nanoscale defects including vacancies, dislocation loops and precipitates, and makes materials brittle and more susceptible to fracture [1]. Currently, the irradiation embrittlement of pressure vessels in nuclear reactors is evaluated by ductilebrittle transition temperature (DBTT) obtained in Charpy impact tests. However, the stock of Charpy specimens preinstalled in the reactors is diminishing and nondestructive evaluation of the irradiation embrittlement has become an urgent matter of study. Recently, we measured magnetic minor hysteresis loops of some neutron irradiated Fe-Cu-Ni-Mn model alloys with high Ni content to investigate the influence of neutron irradiation on magnetic properties [2]. It was found that minor-loop coefficients which are obtained from power-law relations between minor-loop parameters and are sensitive to internal stress [3], decrease with fluence. This shows the reduction of internal stress during neutron irradiation and was explained as being due to a compensation of internal stress of dislocations by Cu precipitates grown around the dislocations. Nevertheless, dependence of elemental content on the coefficients as well as their relation with mechan1 Corresponding Author: Satoru Kobayashi, NDE and Science Research Center, Iwate University, 4-3-5 Ueda, Morioka 020-8551, Japan, E-mail:
[email protected] .
38
S. Kobayashi et al. / Evaluation of Irradiation Embrittlement in Fe-Cu-Ni-Mn Model Alloys
Table 1. Chemical compositions of measuring samples. (wt %) Sample
Cu
Ni
Mn
OV4
0.05
0.8
1.6
OV5
0.05
1.6
1.6
OV6 OV7
0.1 0.1
0.8 1.6
1.6 1.6
OV8
0.05
1.6
1.6
OV17
0.2
1.6
1.6
P
Si
0.025
0.5
Table 2. Neutron irradiation conditions in this study. Fluence Φt (1019 n cm−2 )
Effective fluence Φteff (1019 n cm−2 )
Flux φ (1012 n cm−2 s−1 )
Flux regime
T29
0.89
high
0.44
0.44
T30
0.07
low
0.02
0.07
T31 T32
0.72 0.26
high intermediate
0.06 0.02
0.07 0.04
ical properties were not investigated in detail. In this paper, we study the influence of Cu and Ni contents on minor hysteresis loops in neutron-irradiated Fe-Cu-Ni-Mn model alloys.
1. Experimental Neutron-irradiated tensile test samples with dimensions of 24 × 5 × 0.5 mm 3 were prepared by Odette group of University of California Santa Barbara (UCSB). Fe-Cu-NiMn model (OV) alloys with variable combinations of Cu and Ni contents listed in Table 1 were neutron irradiated at 290 ◦ C. We examined four irradiation conditions with fluence Φt up to 0.44 × 10 19 n cm−2 and with neutron flux φ in the range 0.07-0.89 × 10 12 n cm−2 s−1 as listed in Table 2. A set of magnetic minor hysteresis loops with various field amplitudes H a was measured at room temperature using a closed magnetic circuit with a sample sandwiched between two magnetic yokes. A cyclic magnetic field with a frequency of 1 Hz and H a up to 6 kA/m was applied along the long axis of the sample. Our analysis showed that there exist several power-law relations between minor-loop parameters in a limited range of Ha in which irreversible movement of Bloch wall mainly contributes to magnetization [3]. From the relations, minor-loop coefficients in proportion to internal stress were determined. In this study, we paid attention to the minor-loop coefficient W F0 , obtained from the power-law relation, given by ∗ nF Ma ∗ 0 WF = WF , (1) Ms where Ma∗ and WF∗ are magnetization and hysteresis loss of a minor hysteresis loop and Ms are saturation magnetization [3]. From least-squares fits of W F∗ − Ma∗ curves to equation (1), the exponent of n F = 1.70 ± 0.03, which is independent of chemical compositions and neutron fluence, as well as W F0 were determined. Here, minor loops
S. Kobayashi et al. / Evaluation of Irradiation Embrittlement in Fe-Cu-Ni-Mn Model Alloys
39
with μ0 Ma∗ = 0.3−1.3 T were used for the fits. The obtained coefficient was typically averaged over 2 - 3 samples for each alloy-irradiation condition and an experimental error of WF0 mainly results from the sample dependence. To compare W F0 obtained with various neutron fluxes, an effective neutron fluence t Φeff , given by Φ teff = Φt (φr /φ)1/2 , was introduced [2,4]. Here, φ r is a reference flux and φr = 0.89 × 10 12 n cm−2 s−1 was assumed. This equation was originally proposed to normalize a flux-dependent change of yield strength [4] and is also useful for magnetic properties; on the Φ teff scale, all minor-loop coefficients obtained for various neutron fluxes fall in the same smooth curve, although lower flux tends to shift the coefficients to lower Φt [2].
2. Results and Discussion Figure 1 shows WF0 as a function of Φ teff . For all OV samples, the behaviour of W F0 seems to be classified into two groups. One is a behaviour seen for OV6 and OV7 that W F0 increases at low fluence, shows a maximum around Φ teff = 0.05 × 10 19 n cm−2 , and then gradually decreases with fluence. The other is a behaviour that W F0 shows a monotonic decrease with fluence (OV5, OV8, OV17) or is almost constant against fluence (OV4). For OV5, OV7, and OV17, both Ni and Mn contents are 1.6 wt% and only the Cu content is different from each other. The decrease of W F0 after irradiation to Φ teff = 0.44 × 10 19 n cm−2 is proportional to Cu content and is most pronounced for OV17 with 0.2 wt% Cu.
Figure 1. WF0 as a function of effective neutron fluence.
On the other hand, a behaviour of W F0 is also influenced by Ni content. For OV4 and OV6 with 0.8 wt% Ni, W F0 is weakly dependent on fluence and the decrease after
40
S. Kobayashi et al. / Evaluation of Irradiation Embrittlement in Fe-Cu-Ni-Mn Model Alloys
irradiation is largely reduced compared with that for OV5 and OV7 with 1.6 wt% Ni, respectively. There observations clearly show that the higher level of Cu and Ni inclusion enhances the decrease of internal stress during neutron irradiation. Note that Si inclusion also seems to enhance a decrease in W F0 after irradiation when data for OV5 and OV8 are compared. The effects of Si inclusion on minor-loop properties are subjects for further study. We now examine a relation of W F0 to yield strength σy obtained by tensile tests performed by UCSB group. Figure 2 shows relations between W F0 and a change in yield strength Δσy for all fluences. Since Δσ y generally increases with fluence, higher Δσ y corresponds to that for higher Φ teff . For all OV samples, WF0 is almost constant or linearly decreases against Δσy . Moreover, the higher Cu and Ni contents the larger a change both in WF0 and Δσy . This correlation implies that a decrease in W F0 originates from the same irradiation mechanism as that for the increase of yield strength.
Figure 2. Relation between WF0 and Δσy at all measuring fluences.
For all materials, neutron irradiation induces changes in mechanical properties. These changes are primarily due to the formation of irradiation defects such as Cu rich and Cu-Mn-Ni precipitates [5]. Since these defects act as obstacles to the movement of Bloch wall, minor-loop coefficients will increase with fluence and Cu and Ni contents. However, WF0 rather decreases with fluence, whereas for some OV samples a peak appears at low fluence. This implies the presence of two irradiation mechanisms that affect magnetic properties; the first mechanism is due to the formation of irradiation defects in the matrix and contributes to an increase in minor-loop coefficients and the other is a mechanism that contributes to their decrease. One of possible mechanism to explain such decrease is the preferential formation of Cu rich and/or Cu-Mn-Ni precipitates on dislocations [6,7]; precipitates are preferentially formed on dislocations to minimize the elastic energy and reduces the internal stress around the dislocations. With increasing Cu and Ni contents, the volume fraction of precipitates also increases [5]. This would enhance the precipitation around the dislocations, resulting in a large decrease of W F0
S. Kobayashi et al. / Evaluation of Irradiation Embrittlement in Fe-Cu-Ni-Mn Model Alloys
41
for OV17 with high Cu and high Ni contents. This enhanced precipitation, on the other hand, makes the material mechanically harder [1], which is reason why W F0 is inversely proportional to Δσ y . In conclusion, we have shown that the minor-loop coefficient is roughly in inverse proportion to yield strength, which is an important mechanical property related with irradiation embrittlement. This result clearly shows that magnetic method using minor hysteresis loops is useful for nondestructive evaluation of irradiation damage in nuclear reactor pressure vessels.
Acknowledgements This research project has been conducted under the research contract with the Japan Nuclear Safety Organization (JNES). We thank Prof. G. R. Odette of UCSB for allowing us to measure neutron irradiated samples.
References [1] [2] [3] [4] [5] [6] [7]
G. R. Odette, G. E. Lucas, Radiat. Eff. Def. Solids 144 (1998) 189. S. Kobayashi, H. Kikuchi, S. Takahashi, K. Ara, Y. Kamada, Studies in Applied Electromagnetic and Mechanics 28 (2007) 217. S. Takahashi, S. Kobayashi, H. Kikuchi, Y. Kamada, J. Appl. Phys. 100 (2006) 113908. G. R. Odette, T. Yamamoto, D. Klingensmith, Philos. Mag. 85 (2005) 779. S. C. Glade, B. D. Wirth, G. R. Odette, P. Asoka-Kumar, J. Nucl. Mater. 351 (2006) 197. S. Takahashi, H. Kikuchi, K. Ara, N. Ebine, Y. Kamada, S. Kobayashi, M. Suzuki, J. Appl. Phys. 100 (2006) 023902. M. K. Miller, K. F. Russell, M. A. Sokolov, R. K. Nanstad, J. Nucl. Mater. 361 (2007) 248.
42
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-42
Analysis of Barkhausen Noise Characteristics and Mechanical Properties on Cold Rolled Low Carbon Steel Hiroaki KIKUCHI a,1, Tomoki KOSHIKA a , Tong LIU a , Yasuhiro KAMADA a, Katsuyuki ARA a, Satoru KOBAYASHI a and Seiki TAKAHASHI a a NDE & SRC, Faculty of Engineering, Iwate University, 4-3-5 Ueda, Morioka, Iwate, 020-8551, Japan
Abstract. Low carbon steel specimens cold rolled at ratios of 0 - 40 % have been examined comprehensively by magnetic Barkhausen noise (MBN) method, and their microstructure were studied by transmission electron microscope. In order to correlate MBN parameters with those mechanical properties, Vickers hardness and ductile-brittleness transition temperature (DBTT) were also evaluated. MBN energy and rms voltage rise rapidly with cold rolling below 10 %, and saturate at higher rolling ratio. This phenomenon is attributed to the combined effects of cell texture and dislocation density. It is also found that good correlation between MBN parameters and Vickers hardness, DBTT. Keywords. Barkhausen noise, Microstructure, Vickers hardness, DBTT
1. Introduction Magnetic Barkhausen noise (MBN) has been widely used to study the ferromagnetic materials nondestructively and there have been investigations of MBN changes under various conditions including fatigue, irradiation, stress and so on [1-3]. It has been proved to be sensitive to grain size, composition, hardness and so on [4, 5]. Therefore, this method is becoming a potential tool for many nondestructive evaluation (NDE) applications. However, the effect of microstructure changes induced from cold rolling on MBN has been rarely investigated. Though Atherton’s group has studied MBN properties in cold rolled nuclear vessel steel [6], their specimens possessed an easy axis in the unrolled state as a result of crystallographic texture, which made the exclusive study of rolling texture by MBN method very difficult. For practical uses, it is important to investigate that effect and a relation between MBN parameters and mechanical properties. In this work, low carbon steel plates with negligible crystallographic texture before deformation by cold rolling were investigated to understand the origin of MBN dependence on rolling texture, and to correlate those MBN parameters with those mechanical properties. 1 Corresponding Author: Hiroaki Kikuchi, NDE & Science Research Center, Faculty of Engineering, Iwate University, 4-3-5 Ueda, Morioka 020-8551, Japan; Phone:+81-19-621-6350; Email:
[email protected]
H. Kikuchi et al. / Analysis of Barkhausen Noise Characteristics and Mechanical Properties
2. Experimental Procedure
43
Excitation coil
Low carbon steel (S15C) plates were prepared and then annealed at 1173 K for one hour, followed by air-cooling. Then, 50 mm 40 mm 13 mm Fi-Si those steels were deformed by cold rolling 60 mm with different reduction ratios of 0, 5, 10, Fig. 1 Schematic view and dimensions of yoke 20 and 40 %. The steel contains 0.15– probe. 0.20wt.%C, 0.15–0.35wt.%Si, 0.30– 0.60wt.%Mn and Fe in balance. For MBN measurement, five kinds of specimens were ground into the same dimension 40 × 60 × 10 mm3. In order to evaluate ductile-brittleness transition temperature (DBTT) Charpy impact test pieces, 10 × 10 × 55 mm3, were machined from each plate along the rolling direction. Disk specimens were Fig. 2 MBN measurement setup. also prepared to evaluate microstructures by Philips-tecnai 30 transmission electron microscope (TEM). The plate specimens were magnetized parallel to the rolling direction by a triangle wave of 1 Hz using a yoke probe. The yoke probe was composed of a U-type Fe-Si yoke and an excitation coil as shown in Fig. 1. MBN signals were detected by a MBN sensor, i.e., an air-core coil with 305 turns and 10 mmI, attached on the surface of specimens. The measurement system is illustrated in Fig. 2. The original MBN signals were amplified (60 dB), filtered (10-100 kHz), and finally sampled at 380 kHz. The MBN results of each sample were measured 10 times and averaged. The MBN parameters dependencies on the cold rolling ratio were studied in terms of MBN energy and rms voltage. MBN energy, EMBN, and rms voltage, Vrms are defined as follows.
EMBN
T
2
³0 VMBN dt
(1)
1 T 2 (2) ³ VMBN dt T 0 where VMBN is original MBN signal and T is half period of excitation field. The absorption energy of the Charpy impact test pieces was obtained by using the Charpy test machine at temperatures between 200 and 360 K. The ductile-brittleness transition temperature (DBTT) was estimated from the absorption energy temperature dependence of the Charpy impact test pieces [7]. The Vickers hardness of the specimens was also measured using a Vickers hardness meter with a load of 500 g. Vrms
3. Results and Discussion Fig. 3 shows typical time dependent of MBN signals and the excitation current applied to the yoke probe for 0% and 40 % reduction ratio specimens. From these profiles, MBN energy and rms voltage was calculated using equations (1) and (2). MBN parameters were plotted as a function of reduction ratio in Fig. 4. They rise rapidly in
H. Kikuchi et al. / Analysis of Barkhausen Noise Characteristics and Mechanical Properties
MBN energy EMBN (mV2)
480
32 MBN energy rms voltage
400
28
320
24
240
20
160
16
80
rms voltage Vrms (mV)
44
12 0
10
20
30
40
50
Reduction ratio (%)
(a) 0 % reduction ratio
Fig. 4 The relation between MBN energy, rms voltage and reduction rate.
the beginning with reduction ratio below 10%, and then slightly increase above 10% cold rolling. In Artherton’s work [6], cold rolling brought about the increase of MBN parameters. The authors attributed these phenomena to crystalline anisotropy before rolling. In our work, on the other hand, Xray analysis revealed that the crystalline anisotropy is not observable before rolling (b) 40 % reduction ratio and the surface residual stress effect is also Fig. 3 typical time dependent of MBN signal and negligible after a surface grinding process. excitation current applied to yoke probe. Fig. 5 shows the micrograph of TEM observation. One can see that dislocations are distributed homogeneously for 0% cold rolling and a large amount of dislocations are generated with the increase of reduction ratio. A cell substructure also comes into being gradually during this rolling process and aligns with the direction parallel to the rolling direction. The formation of rolling texture <110> was observed by X-ray analysis. The dislocation density Uestimated by the Ham method [8] is 5 × 109 cm-2, 2 × 1010 cm-2, and 6 – 10 × 1010 cm-2 for 0%, 5%, and 10% reduction ratio, respectively; for higher reduction, is not shown because of the formation of cell structures, which makes it difficult to estimate a reliable value of U. It is proposed that the increase of MBN parameters is attributed to the combined effects of cell structure and dislocation density. TEM observation reveals that dislocations tend to aggregate at the boundary of cell structure during the cold rolling, and the dislocation density inside the cell texture is relatively low so that the domain wall can come across. Consequently, increases in dislocation density with cold rolling lead to sensitive increases in the domain wall gradient at pinning site, resulting in a larger MBN response up to 10 % reduction ratio. On the other hand, above 10 % increases in dislocation density becomes not significantly, whereas a higher rolling ratio induces a large number of smaller cell structures, namely the boundary area increases, which results in low MBN signal. Therefore, the total MBN response tends to saturate at high reduction ratio. This MBN analysis method shows a potential application in evaluating microstructure changes nondestructively in cold rolled steel. The relations between MBN parameters and mechanical properties, DBTT and Vickers hardness, are shown in Fig. 6. DBTT and Vickers hardness increases as reduction ratio increases due to work hardening. MBN parameters rise rapidly with increasing mechanical parameters below 10 % reduction ratio, and then they increase
45
H. Kikuchi et al. / Analysis of Barkhausen Noise Characteristics and Mechanical Properties
(a) 0 % (b) 5 % (c) 10 % Fig. 5 TEM micrographs showing dislocations in S15C steel.
24
300
22
260
20
220
18
180
16
140 130
140
150 160
170
180 190 200
Vickers hardness (Hv)
MBN energy EMBN (mV2)
340
26
380 340
24
300
22
260
20
220
18
180
16
140 245
14 210
MBN Energy rms voltage
250
255 260
265
270 275
280
rms voltage Vrms (mV)
26 MBN Energy rms voltage
rms voltage Vrms (mV)
MBN energy EMBN (mV2)
380
(d) 40 %
14 285
DBTT (K)
(a) MBN parameters vs. Vickers hardness (b) MBN parameters vs. DBTT Fig. 6 The relations between MBN parameters and mechanical properties, DBTT and Vickers hardness.
gently over 10 % reduction ratio. Though the relation between MBN parameters and mechanical parameters is not simple proportional, MBN parameters shows the increases monotonically as function of mechanical parameters. Thus, these results represent a possibility of NDE for the mechanical properties using the Barkhausen noise technique.
4. Conclusion The MBN and mechanical properties of cold rolled low carbon steel were studied. MBN energy and rms voltage rise sharply in an initial stage of cold rolling and gently over 10% cold rolling ratio. The Vickers hardness and DBTT exhibits the same tendency as MBN parameters. Dislocations increase with the increase of the rolling reduction, which cause the increase of Vickers hardness and DBTT. The formation of cell texture and the changes in dislocation density dominated the MBN properties. Good correlations between MBN parameters and mechanical parameters were derived, which show the Barkhausen technique is a good candidate of NDE for the mechanical properties of cold rolled steel.
References [1] C. C. H. Lo, J. Paulsen and D. C. Jiles, IEEE Trans. Magn., 40 (2004) 2173-2175. [2] S. Palit Sagar, N. Parida, et al., Int. J. Fatigue, 27 (2005) 317-322. [3] V. Moorthy, B. A. Shaw, S. Day, Acta Mater., 52 (2004) 1927-1936. [4] J. Anglada-Riveraa, L. R. Padoveseb, J. Capó-Sáncheza, J. Magn. Magn. Mater., 231 (2001) 299-306. [5] O. Saquet, J. Chicois, A. Vincent, Mater. Sci. Engineering, A269 (1999) 73–82. [6] C. G. Stefanita, L. Clapham, J. K. YI, D. L. Atherton, J. Mater. Sci., 36 (2001) 2795-2799. [7] Y. Kamada, T. Nakano, S.Takahashi, et al., J. Magn. Jpn., 28 (2004) 409–412. [8] R. Ham, Philos. Mag., 6 (1961) 1183–1184.
46
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-46
A Bridge Between NDE and Charpy Impact Testing Seiki TAKAHASHI 1 and Satoru KOBAYASHI NDE and Science Research Center, Faculty of Engineering, Iwate University, Morioka 020-8551, Japan Abstract. Charpy impact test is explained from the viewpoint of the transition of hammer’s energy to the kinetic energy of dislocations. Ductile-brittle transition temperatureT is represented as a simple function of the nucleation energy of dislocations Hn, the dislocation density U, the maximum density of mobile dislocations Uo and the interaction energy of obstacles with dislocations Uob; kT = UobҏUo +(Uo-U)Hn when U< Uo, while kT = UobҏUm when U> Uo, where k is Boltzmann constant and Um is the density of mobile dislocations. The relationship is compared with the experimental results for cold rolled S15C steels and neutron irradiated low and high copper A533B steels of nuclear reactor pressure vessel materials. The experimental results are qualitatively explained by the present model. Keywords. Charpy impact test, dislocations, ductile-brittle transition, plastic deformation, neutron irradiation
1. Introduction Charpy impact test is an useful and reliable method to get information on ductility of materials and has been traditionally used for a long time in the engineering field.[1,2] The surveillance test of nuclear reactor pressure vessels (NRPVs) has been carried out by Charpy impact method and the obtained ductile-brittle transition temperature (DBTT) decides the lifetime of NRPV. The mechanism of age degradation in NRPV has been investigated from the viewpoint of microstructure and it is widely accepted that copper precipitates with size of 2-3 nm, which nucleate and grow by the neutron irradiation, make material brittle.[3,4] On the other hand, the nucleation mechanism has been recently investigated by magnetic method in NRPV material and it was suggested that copper precipitates gathering around dislocations through the elastic interaction also contribute to the degradation.[5] Currently, the degradation in NRPV is evaluated by DBTT obtained by Charpy impact test that is a macroscopic property. Nevertheless, there exist few ideas to connect the macroscopic property with the microscopic one and its physical meaning is vague at present. We need a bridge between the microstructure of irradiation damages and the traditional mechanical properties for the practical use. The relationship between DBTT and magnetic properties has been investigated experimentally and it was found that coercive field increases in proportion to DBTT.[6] Charpy impact method is a destructive test, whereas the magnetic method has a characteristic of non-destructive evaluation. We need the physical model of DBTT to explain the relationship of DBTT with magnetic properties. The purpose of the present 1 Corresponding Author: NDE&Science Research Center, Faculty of Engineering, Iwate University, 4-3-5 Ueda, Morioka 020-8551, Japan; Phone:+81-19-621-6431; Email:
[email protected]
S. Takahashi and S. Kobayashi / A Bridge Between NDE and Charpy Impact Testing
47
study is to give physical explanation for the DBTT and absorption energy from the microscopic viewpoint. In this study, we introduce a dislocation model representing the absorption energy versus temperature and express DBTT by physical properties. The experimental results are analyzed and DBTT and upper shelf energy are explained on the basis of the present dislocation model in the neutron irradiated low carbon steels.
2. Charpy impact test Ductile and brittle states are examined by Charpy impact test in which a hammer accelerated by gravity potential collides with a test piece and the hammer energy lost by the collision is measured. The lost energy is very small in the brittle state, whereas in ductile state the hammer energy is absorbed into the test piece. The metallic materials are brittle at low temperatures but change to ductile above the critical temperature. This critical temperature is called ductile-brittle transition temperature. The value of DBTT depends on the kinds of materials and increases with the progression of degradation. The absorption energy in the ductile state also depends on the degree of degradation and the ductility of materials is therefore evaluated by both DBTT and the upper shelf energy. [1,2] Samples are deformed plastically in the ductile state when a hammer collides. The hammer’s energy is consumed for plastic deformation and is then transformed into thermal energy. Plastic deformation is cause of the nucleation and motion of dislocations from the microscopic viewpoint. On the other hand, in the brittle state dislocations cannot move and the samples are broken down without the dislocation motion.
3. Absorption energy and dislocations In the ductile state, most of a potential energy of a hammer are transferred to a kinetic energy of dislocations during the collision that is the main part of the absorption energy in Charpy impact test. The mechanism of the energy transition depends on the dislocation density. If there exist many dislocations enough to receive the hammer’s energy, the interaction of dislocations with their obstacles decides the energy transition. If dislocations do not exist enough, the hammer’s energy would be consumed for nucleation of dislocations and their kinetic energy. If the energy transformation is adiabatic, though transformation in actual Charpy impact test is not adiabatic, the absorption energy is represented as a step function of temperature as shown in Figure 1. The energy is discontinuously transformed at the transition temperature T. The absorption energy of the step function can be approximately expressed by the equation Eabs = Uo exp[- (U/kT)n] ,
(1)
where n = f. Here, Uo is an upper shelf energy, k is Boltzmann constant and U is the transition energy. The transition temperature T is given by
48
S. Takahashi and S. Kobayashi / A Bridge Between NDE and Charpy Impact Testing
Absorption energy Eabs/ U0
1.2 adiabatic (n=п) 1 n = 50 n = 30 n = 15
0.8 0.6 0.4
static (n = 1)
0.2 0 0
0.5
1
1.5
2
T/T Figure 1. Energy transition processes for n = 1 (static), 15, 30, 50, f (adiabatic) cases.
U = kT
(2)
and is not the same value as the definition of DBTT. Another extreme case of energy transformation is the quasi-static transition where the energy is transformed at the constant temperature near T, during the infinite time. In this case, the absorption energy is written as Eabs = Uo exp[-(U/kT)],
(3)
which is represented in Figure 1. The actual transition in Charpy impact test is represented as a model of the intermediate of two examples, taking an adequate n in Equation (1), and an absorption energy for n = 15, 30, 50 is plotted in Figure 1 as an example. The energy transition in Charpy impact test is explained under supposition that any phase transition does not occur in the temperature range of the measurement. The hammer’s energy is transformed into the kinetic energy of dislocations during the collision. The energy transition is performed perfectly near Twhen the dislocation density is high enough to receive the potential energy and their mean free path is long enough for dislocations to accumulate their kinetic energy. However, there exist a lot of obstacles against the dislocation motion in real materials. The obstacles interact with dislocations and restrict the dislocation motion. The interaction of obstacles with dislocations is represented as an interaction energy Uob that depends on the strength of the interaction, the density and distribution of obstacles. Dislocations themselves act as the obstacles, make the mean free path short and the number of mobile dislocations small near and above T. When the dislocation density is not enough to receive the hammer’s energy, the dislocations would be nucleated by the energy supplied from the hammer during the collision. The absorption energy is written as, neglecting the obstacle effect, Eabs = Uo exp[- ((Uo - U)Hn/kT)n] ,
(4)
where U is the dislocation density before the collision, Hn is the nucleation energy of dislocations per unit length and Uo is the maximum dislocation density to receive the
S. Takahashi and S. Kobayashi / A Bridge Between NDE and Charpy Impact Testing
49
potential energy of the hammer. Generally, materials include obstacles and both obstacles and the dislocation density contribute to the absorption energy. When U is lower than Uo, dislocations with density of Uo-U should be nucleated and the absorption energy would be represented by Eabs = Uo exp[-((Uob̓ Uo +(Uo - U)Hn)/ kT)n]
(5)
On the other hand, when U is higher than Uo, the absorption energy is represented as Eabs = Uo exp[-(Uob̓ Um/ kT)n].
(6)
Here, Um is the density of mobile dislocations that is lower than Uo. Uo is the maximum of Um. The dislocation density is not included in Equation (6) explicitly but Uob is related to the density and distribution of dislocations, because dislocations play an important role as obstacles even in the initial stage of plastic deformation. The upper shelf energy Uo depends on the density of mobile dislocations and their mean free path in the collision. Uo is the kinetic energy of dislocations; i.e.
Uo F't
p2 U m ҏ, 2m
'( pU m ) p
m
(7)
U m 'p p'U m 'x 't
,
(8)
,
(9)
where p is the momentum of a dislocation per unit length and depends on the mean free path x. m is the effective mass of a dislocation and F is the force acting on dislocations during collision time 't. Dislocations are accelerated during 't. When x is long enough, the momentum would become large. If the density of mobile dislocations Um is small and x is short, 't would become short and the material is brittle. Uo depends on Um. The strength of interaction energy and the test temperature restrict the density Um; dislocations get over obstacles through the thermal activation process and the external force F that is decided by the external conditions of a hammer.
4. Comparison with experimental results The relationship between DBTT and dislocations has been investigated in S15 C steel, where the dislocations are induced by cold rolling with 0, 5, 10, 20 and 40% strain. The chemical composition of S15C steel is listed in Table 1. The absorption energy was measured by use of Charpy impact test pieces with the standard size of Table 1.
Chemical compositions of S15C steel.
S15C
C
Si
Mn
Fe
wt.%
0.16
0.20
0.44
balance
50
S. Takahashi and S. Kobayashi / A Bridge Between NDE and Charpy Impact Testing
10×10×55 mm. The impact tests were carried out with a pendulum of 27.6 kG and lift angle of 138.5° in the temperature range of 200-363 K. Five V-notched Charpy samples were tested at each temperature and both the largest and smallest values of absorption energy were eliminated when averaging the data. Figure 2 shows the temperature dependence of absorption energy. The lines are obtained by fitting the experimental results to Equation (1). The value of n changes from 15 to 30 depending on plastic deformation; it increases with rolling reduction initially, takes the maximum for 20% rolling reduction and decreases above 40% reduction. The dislocation density is not enough before cold rolling, whereas obstacles are present. The hammer’s energy would be consumed by the two processes; the nucleation of dislocations and climbing over obstacles. The dislocation density becomes enough by 5% rolling reduction and the process becomes only climbing of obstacles. The value of n increases from 15 to 30. The dislocations play the roll of obstacles above 20% rolling reduction. The pinning processes of dislocations increase and the value of n decreases from 30 to 15. The value of DBTT was obtained experimentally as the temperature at which the upper shelf energy becomes a half. Figure 3(a) shows the relation between DBTT and rolling reduction, which is compared with the calculated value of T and the upper shelf 250
0% 5% 10% 20% 40%
Absorption energy (J)
200
150
100
50
0 180 200 220 240 260 280 300 320 340 360 380
Temperature(K)
Figure 2. Temperature dependence of absorption energy in cold rolled S15C steel. The carved lines are calculated results n = 15, 31, 61, 25 and 11 correspond to H = 0, 5%, 10%, 20%, and 40% in strain, respectively.
(a)
180
270
160
260
140
250 120 240 100 230
600
0
10
20
30
40
Rolling reduction (%)
50
U0
DBTT, T (K)
280
200
Coercive field Hc (A/m)
290
(b) 500
400
300
200 240
250
260
270
280
290
DBTT (K)
Figure 3. (a) DBTT and theoretical values of T and Uo as a function of rolling reduction in S15C steel. The solid and open circles, and triangles denote DBTT, T and Uo, respectively. (b) The relation between DBTT and coercive field of S15C steel.
51
S. Takahashi and S. Kobayashi / A Bridge Between NDE and Charpy Impact Testing
Table 2.
Chemical compositions of A533B steel.
A533B
C
Si
high Cu
0.19
0.19
1.47
0.16
0.64
0.51
0.14
balance
low Cu
0.19
0.18
1.46
0.05
0.64
0.50
0.14
balance
Table 3.
Mn
Cu
Ni
Mo
Cr
Fe
n, T and U0 of A533B steels before and after neutron irradiation.
T.
n
A533B
Uo (J) 223 ± 75
high Cu (before)
7±2
232 ± 5
(after)
4±2
312 ± 30
low Cu (before)
11 ± 4
215 ± 6
174 ± 27
(after)
12 ± 4
238 ± 4
153 ± 11
181 ± 50
energy Uo. The relation between DBTT and coercive field obtained in our previous work[6] is also given in Figure 3(b). DBTT has been measured before and after the neutron irradiation in NRPV A533B steels with low and high copper contents. Their chemical contents are shown in Table 2. The neutron radiation was performed at 563 K in helium atmosphere in a 50 MW nuclear reactor of Japan Materials Testing Reactor(JMTR). The radiation effect that yields the brittleness has been examined after the neutron fluence to 5 × 1019 cm-2. The number of test pieces is limited to two for each temperature. Figure 4(a) shows the temperature dependence of absorption energy in high copper A533B steel. The lines are obtained by fitting the experimental results to Equation (6). The values of n , Tand Uo ̓change by the neutron radiation, from 7 ± 2 to 4 ± 2, 232 ±5 K to 312± 30 K and 223±75 J to 181± 50 J, respectively as listed in Table 3. Figure 4(b) shows the temperature dependence of absorption energy in low copper A533B steel. The values of
250
250
(a)
high Cu
unirradiated
Absorption energy (J)
Absorption energy (J)
300
200 150 100
irradiated
50 0 150
200
250
300
350
Temperature (K)
400
450
(b)
low Cu
200
unirradiated
150
irradiated 100
50
0 150
200
250
300
350
400
450
Temperature (K)
Figure 4. Temperature dependence of absorption energy in A533B steel with (a) high copper and (b) low copper contents, before and after neutron irradiation to a fluence of 5 × 1019 cm-2. The solid lines through the data shows the least squares fits.
52
S. Takahashi and S. Kobayashi / A Bridge Between NDE and Charpy Impact Testing
n ,Tand Uo ̓change by the neutron radiation from11 ± 4 to 12 ± 4, 215 ± 6 K to 238 ± 4 K and 174 ± 27 J to 153 ± 11 J, respectively as listed in Table 3. The large deviation of n , Tand Uo is attributed to the lack of data points and the shortage of test pieces. Neutron radiation would not exert any remarkable influence on the distribution of dislocations as well as the dislocation density but on the interaction energy Uob. The change of properties due to neutron radiation is smaller in low copper A533B steel than in higher copper one.
5. Discussion In cold rolled S15C steel, the transition temperatures DBTT and T show similar change against rolling reduction though the value of DBTT is slightly larger than that of T as shown in Figure 3. The obstacles to the dislocation motion are dislocations themselves and their interaction would be proportional to the applied stress. The value of T shows a gentle increase from 5% to 40% in rolling reduction, whereas it increases rapidly from 0 to 5% in rolling reduction. The upper shelf energy U0 decreases monotonically from 0 to 40% reduction. The monotonic decrease of U0 indicates that the mean free path would decrease and the density of mobile dislocations would not change remarkably. The dislocation density of A533B steels is higher than 1010 cm-2 before neutron radiation and dislocations make cell structure. The dislocations that do not contribute to the cell structure can move the same distance as the size of a cell, because there exist little dislocations inside of the cell. Therefore, the mean free path would be large, whereas the value of Um is small. Recently, it was suggested by the magnetic method that the copper precipitates and dislocation loops created by neutron radiation would gather around dislocations and disturb the dislocation movement.[5] Since copper precipitates have stress field and edge dislocations include both compressive and repulsive stress field, copper precipitates gathering around the dislocations would compensate the stress field of dislocations in order to reduce the elastic energy. The copper precipitates strongly disturb the dislocation movement and makes high copper A533B steel brittle. On the other hand, copper precipitates inside of cells also disturb the dislocation movement and make the mean free path x decrease. Since the value of Um would not change by the neutron radiation, the value of Uo decreases as is listed in Table 3. Copper precipitates make the value of Uob increase and their inhomogeneous distribution makes the distribution of Uob wide. This results in a decrease of n due to neutron radiation in the high copper A533B steel. The amount of copper precipitates nucleated by neutron radiation is small in A533B steel with low copper content in comparison with that for high copper content. The change of T (DBTT) is 18 ± 5 K in low copper A553B steel that is much smaller than 80 ±30 K in high copper A533B steel. The difference of the change in T is attributed to the number of obstacles, which decide the value of Uob. The value of n does not change remarkably by the radiation in low copper A533B steel. This result indicates that the obstacles distribute homogeneously. The change of Uo due to neutron radiation in low copper A533B steel is also smaller than that of the high copper A533B one, being consistent with the results of T. The main obstacles to dislocation motion in A533B steels are copper precipitates and their amount depends on the copper contents. DBTT gives us the direct information about ductility and brittleness from a macroscopic viewpoint and can be qualitatively explained by the dislocation theory. On
S. Takahashi and S. Kobayashi / A Bridge Between NDE and Charpy Impact Testing
53
the other hand, dislocations also interact with magnetic domain walls and influence their movement. According to earlier theory for micromagnetism, arrangement of magnetization is determined so as to minimize magnetic Gibbs free energy consisting of exchange energy, magnetocrystalline anisotropy energy, magnetostatic energy and magnetoelastic energy.[7] In ferromagnetic materials including dislocations, the Gibbs free energy is lowered when domain walls are located at dislocations and dislocations act as obstacles to the domain wall motion, yielding changes in magnetic properties. Therefore, both magnetic and mechanical properties have an intimate connection with each other through dislocations as is seen in the simple relation between DBTT and coercive field in Figure 3(b). Such connection is also true for NRPV steel irradiated by neutron where various kinds of lattice defects such as precipitates which disturb dislocation motion are formed; these irradiation defects interact with domain walls as in the case of dislocations.[7-9] However, the crucial difference between these properties is the fact that magnetic properties can be obtained by nondestructive measurements whereas Charpy impact test is destructive one. The practical application of magnetic methods to NDE is therefore expected for the pressure vessel of nuclear reactors exposed to neutron radiation.
Acknowledgements The authors express thanks to Dr. Y. Kamada, for the Charpy impact test measurement, Dr. H. Kikuchi, K. Ara and N. Ebine for the operation of the nuclear reactor. This research was supported by a Grant-in-Aid for Scientific Research (S), Grant No. 14102034, from the Ministry of Education, Culture, Sports, Science and Technology of Japan.
References [1] E. R. Parker, in Brittle Behavior of Engineering Structure, (John Wiley & Sons, 1957). [2] D. Francois, in From Charpy to Present Impact Testing, (ESIS Publication, 2002) [3] J. Koutský and J. Kocík, in Radiation Damage of Structural Materials, (Elsevier Science Publishers, 1994). [4] G. R. Odette and G. E. Lucas, JOM 53 (2001) 18. [5] S. Takahashi, H. Kikuchi, K. Ara, N. Ebine, Y. Kamada, S. Kobayashi and M. Suzuki, J. Appl. Phys. 100 (2006) 023902. [6] S. Takahashi, S. Kobayashi, Y. Kamada, H. Kikuchi,, J. Appl. Phys. 100 (2006) 113908. [7] H. Kronmüller and M. Fähnle, in Micromagnetism and the Microstructure of Ferromagnetic Solids (Cambridge, 2003). [8] L. J. Dijkstra and C. Wert, Phys. Rev. 79 (1950) 979. [9] J. B. Goodenough, Phys Rev. 95 (1954) 917.
54
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-54
ND-materials characterization of neutroninduced embrittlement in German nuclear reactor pressure vessel material by micromagnetic NDT techniques Gerd DOBMANN1, Iris ALTPETER1, Melanie KOPP1, Magdalena RABUNG1, and Gerhard HÜBSCHEN1 1 Fraunhofer IZFP, Germany
Abstract. Depending on the neutron fluence and the special design of the pressure vessel of nuclear power plants (NPP) the microstructure of the steels change by neutron induced embrittlement. Embrittlement is on the basis of vacancies and Curich precipitates which in the size range of 1-3 nm contribute with coherent residual stresses of the 3rd kind to an increase in hardness and strength (yield strength and tensile strength) as well as with a reduction of the upper shelf value of Charpy energy and a shift in the brittle-to-ductile transition temperature to higher temperatures. Micromagnetic investigations sponsored by the German minister of economics were performed at full Charpy specimen and material of the last generation of German NPP in order to characterize the material degradation. The contribution reports to the results obtained by the application of the Micromagnetic-, Multiparameter-, Microstructure-, and stress-Analysis (3MA) and the magnetostrictive excitation of ultrasound using an EMAT. Both technologies document potential to be further developed to an in-service inspection technique.
Keywords. Neutron irradiation, embrittlement, pressure vessel material, micromagnetic NDE techniques, multiple regression, calibration
Introduction In the year 2003 IZFP has participated in the EURATOM project GRETE where the characterization of neutron degradation of pressure vessel material was one project task. Materials came from surveillance and irradiation programs. All specimens were investigated in the hot cells of the research reactor in Petten, the Netherlands. The specimens were half Charpy specimens obtained after the performance of the Charpy impact energy test, i.e. the specimen have had plastic deformation and residual stresses
G. Dobmann et al. / ND-Materials Characterization of Neutron-Induced Embrittlement
55
as disturbing influences. Concerning micromagnetic NDT techniques proposed by IZFP the effects strongly influence the results. However, performing the so-called 3MA-approach (Micromagnetic, Multiparameter, Microstructure and stress Analysis) [1] after calibration correlation coefficients in the 0.98 range were obtained with a residual standard deviation of 16°C when, for instance, the shift – compared with the non-irradiated material state - of the ductile to brittle transition temperature 'T09 was predicted. When ISO-v-notched specimen, for instance according to the ASTM standard A370 are tested in the Charpy impact test in order to evaluate the Charpy impact energy as function of temperature, each half of the broken specimen has shear lips in the fracture plane, i.e. the broken specimen shows a broadening compared with the initial state. The broadening is defined as the difference value between the specimen width with shear lips after break and the initial width value. T09 is derived from the fitted and averaged Charpy impact energy versus temperature curve as the special temperature where the broadening meets the value 0.9mm. However, a verification test of the approach by independently selected specimen resulted in much larger deviations because of the above mentioned disturbing effects [2, 3].
1. Material Selection
Figure 1. Neutron fluence in a German NPP of the last generation as function of lifetime
As directed by the German minister of economics – responsible for nuclear safety – a project was performed where the objective in a feasibility study was to demonstrate the potential of micromagnetic NDT techniques to characterize the material degradation by neutron irradiation when the neutron fluence is much smaller compared to the former discussed European project. Background is that in Germany (see Figure 1), according to the German codes, the design lifetime is 32 years and the fluence is restricted to values of 5×1018 n/cm2 (Energy >1MeV). This design end-of-life value (green curve in Figure 1.) is one order
56
G. Dobmann et al. / ND-Materials Characterization of Neutron-Induced Embrittlement
in size smaller than in other countries and is obtained by a much larger gap between PV-wall and core internals in the German design compared with others. When the real behavior of the material is discussed resulting from fluence measurements then the fluence curve follows (in an extrapolation) the red curve. After 48 years of full power service only a value of 3.35×1018 n/cm2 is obtained documenting also the potential of a possible lifetime extension. The materials selected to perform the non-destructive tests were from the two steel types 22NiMoCr37 and 20MnMoNi55. The important contents of the elements Cu, P and Ni are indicated in Table 1 where also the available fluence values are documented. As can be seen, the specimens named P16 with the highest Cu, P, and Ni-content have the highest fluence values, i. e. they have the highest degree in degradation. Table 1 Steel grades selected for materials characterization Indication
P140
Weld Material /Base Material
Cu [%]
WM
0,07
P [%]
Ni [%]
Fluence [n/cm²]
0,009
0,9
3,72E+18 7,55E+18 1,04E+19 3,71E+19
P141
BM
0,06
0,008
0,8
3,78E+18 7,66E+18 1,05E+19
P16
WM
0,08
0,012
1,7
4,15E+18 8,04E+18 1,16E+19 5,22E+19
According to Figure 2 the materials P 16 and P 141 show normal behavior, i.e. an increase of the of the shift (dt41) of the brittle-to-ductile transition temperature with fluence, whereas the P 140 material documents a recovery annealing, first increasing then decreasing. The arrows in Figure 2 indicate the tendency. In this case the transition temperatureT 41 in contrast to T09 is discussed which is derived from the fitted and averaged Charpy impact energy curve as function of temperature exactly where the curve meets the value of 41J. P16 – weld metal P 16 WM
P 141 BM
P140 – weld metal
P141- base metal P 140 WM
Neutron fluence times 10E18 Figure 2. Shift in the brittle-to-ductile transition temperature (dt41) as function of the fluence (abscissa) of the three materials
G. Dobmann et al. / ND-Materials Characterization of Neutron-Induced Embrittlement
57
2. Measurements with 3MA Techniques and Correlation with Toughness Parameters The 3MA measurements were performed in the hot cell of AREVA whereas only the magnetic yoke transducer was inside the hot cell and the electronic equipment outside. The Charpy specimens were handled by a manipulator. A special adaption piece made by an Al-alloy was applied to guarantee reproducibility in positioning of the specimen at the yoke pole shoes. The 3MA-approach is described in detail elsewhere [1]. However, a short explanation is given here (Figure 3). With 3MA different micromagnetic quantities are measured. These are derived by analysis of the magnetic Barkhausen noise M(Ht), the incremental permeability μ(Ht) as function of a tangential magnetic field Ht which varies as function of time (t) according to a sinusoidal time function. In Figure 3, in a sketch, the different measuring quantities are illustrated: In the middle a magnetic hysteresis (induction B(H) versus the magnetic field H), in the upper left part the Barkhausen noise M which is an electrical voltage received by integrating the magnetic flux excited by Bloch wall jumps and rotational processes of the magnetization vectors of the domains. In the upper right part the incremental permeability which is the inclination of the small inner loop (see hysteresis) 'B/'H and proportional to the impedance of an eddy current coil superimposing to the hysteresis loop the small incremental magnetic field 'H of a frequency, at minimum, a factor 10 higher than the hysteresis frequency. H, respectively Ht are measured in A/cm, the time t in s and the induction B in T. In the lower left part of Figure 3 the harmonic analysis of the tangential field strength is shown and how, for instance, a distortion factor K can be derived by measuring the odd harmonics up to order of seven. The lower right part of Figure 3 documents an additionally performed eddy current impedance measurement with three different frequencies. The 3MA-approach correlates a target value like, for instance, the dt41 transition temperature shift in a multiple regression model with the micromagnetic measuring quantities and estimates the unknown parameters of the model by applying a least squares algorithm.
Figure 3. The 3MA approach
58
G. Dobmann et al. / ND-Materials Characterization of Neutron-Induced Embrittlement
In the least squares algorithm only one part of the set of specimens is used for calibration of the model, the other independently selected part is applied to check the quality of the model (verification test).
Figure 4. 3MA result at the P16 specimens
In Figure 4 as one result the shift in the brittle-to-ductile transition temperature (dT41) is compared with the predicted values by 3MA. The red colored dots indicate the calibration specimens, the green colored the verification specimens. The regression coefficient from the calibration is 0.93 with a residual standard error of 12.8°C. However, because of the inhomogeneous microstructure in the weld material P16 (multiple-path welding under submerged arc) the residual standard error concerning the verification specimens 24.8°C is nearly a factor 2 larger. In the base material the obtained standard errors are much smaller. This is documented in Figure 5 in case of the material P 141. The regression coefficient after the calibration is 0.986; the residual standard error in the verification is only 1.2°C.
Determination of the shift of the ductile to brittle transition temperature dT41 by the 3MA-technique Base material P141
r2 = 0.986 Standarderror = 0.35 (Calibration) Standarderror = 1.2 (Verification)
Figure 5. 3MA result at the P141 material
The future plan is to develop an ISI inspection technology to examine the pressure vessel from the inner side by a 3MA approach. However, in that case the inspection has to be performed through the austenitic stainless steel cladding which itself has certain G-ferrite content, a ferromagnetic phase. Therefore the influence of the cladding on a micromagnetic technique like Barkhausen noise was investigated. Figure 6 documents the result. Shown are Barkhausen noise profile curves [1] which are obtained when the
G. Dobmann et al. / ND-Materials Characterization of Neutron-Induced Embrittlement
59
received electrical voltage (ordinate) as time signal in a (x,y)-presentation on the oscilloscope is visualized versus the time signal of the magnetic field (abscissa). Even through the 10 mm thick austenitic plate the Barkhausen noise from the ferritic plate can be recorded. The thickness of the austenitic plate influences the inspection mainly by a larger lift-off effect. However, there is also a higher eddy current damping because of the electrical conductivity of the cladding.
Figure 6. Barkhausen-noise M as function of a tangential magnetic field Ht at a ferritic plate (left), through 8 mm austenitic (middle) and 10 mm austenitic (right) plate with G-ferrite simulating the cladding
3. Magnetostrictive Electromagnetic Excitation of Ultrasound (EMUS) G. Ahlers had previously proposed to excite a standing, low frequency (10 kHz, O=320 mm) ultrasonic wave by a magnetostrictively working electromagnetic acoustic transducer (EMAT) [4] in the interface between the austenitic cladding and the ferritic material of the PV wall propagating in thickness direction. In Figure 7 the principle of such an inspection is shown which up to now is not yet realized for ISI-technology. A dc- or low frequency ac-electromagnet magnetizes locally the pressure vessel wall from the inner side through the cladding. A high-frequency (HF)-current tone burst is exciting a HF-eddy-current coil; the magnetic field is controlled by a Hall probe. The principle was investigated using cladded test pieces. Figure 8 gives a view on the experimental set-up using a Bruker water-cooled laboratory electro-resistance dcmagnet with a maximum magnetic induction field of 1.5 T. transmitter coil
receiver coil
poleshoes of electromagnet
Figure 7. Principle of the magnetostrictive excitation of a standing wave in thickness direction
Figure 8. EMAT transmitter-receiver prototype transducer at a cladded test piece
60
G. Dobmann et al. / ND-Materials Characterization of Neutron-Induced Embrittlement
The HF-coil was designed as transmitter receiver coil with adopted coil windings; the burst frequency was 50 kHz. The cladded test piece was set-up at the pole shoes of the laboratory magnet. It was shown that G-ferrite changes in the cladding doesn’t change the results very much. This is documented in the Figures 9 and 10. In the case of Figure 9 the standing wave was excited in a ferritic plate with wall thickness 30 mm but with a lift-off of the transducer of 8 mm whereas in Figure 10 the test piece was a 30 mm thick cladded material with a cladding thickness of 8mm. Insonification was performed from the cladded surface. The electrical signals were obtained by an excitation with a burst length of 10 cycles of a 50 kHz tone-burst at a magnetic field strength of 260 A/cm. It is obvious; the cladding is mainly influencing the signal with a lift-off effect. There were also investigations concerning the influence of the inhomogeneous microstructure of a ferritic butt weld beneath the cladding on the magnetostrictive excitation. This situation occurs at pressure vessels along an inspection path in the direction of the circumferential welds. By scanning with the EMAT along such a weld and measuring the resonance amplitude as function of the different positions only a standard deviation of < 4%, compared with the average value, has been observed. This reflects the change of magnetostriction with the microstructure of a multilayer submerged arc weld. This value has to be compared with the measuring effect obtained at neutron irradiated material. Because the dynamic magnetostriction is sensitive to lattice defects it was assumed that the resonance amplitude of the standing wave also reflects the neutron embrittlement and first experiments were also performed with a special designed magnetostrictive transducer at Charpy specimen in the hot cell of AREVA in order to principally document the potential.
Figure 9. Magnetostrictive excitation of the standing wave in a ferritic plate, lift off of the transducer 8 mm in air (abscissa is the time scale, the ordinate is the electrical voltage induced in the EMAT by the ultrasonic wave)
Figure 10. Magnetostrictive excitation of the standing wave excited beneath the cladded surface, cladding thickness 8 mm (abscissa and ordinate like in Figure 9)
The EMAT especially optimized to test the small geometry of Charpy specimens operates at 1.2 MHz. The echo sequence of the excited standing wave was recorded by varying the superimposed magnetic field. The time signal was time gated (Figure 11) and in the gate the peak amplitude was registered. The so obtained measuring quantity was named E60, indicating that the measurement was performed at the 60% amplitude level of the maximum magnetic field strength. This is an operating point of the magnetic field at which the magnetostrictive excitation has not yet obtained its maximum. It is obvious, at the higher operating frequency of 1.2 MHz the efficiency of transduction and receiving is better than in the lower frequency range (10 kHz) used at
G. Dobmann et al. / ND-Materials Characterization of Neutron-Induced Embrittlement
61
the plates. In Figure 12 by testing the P16 material the measuring quantity E60 shows a linear decreasing with the dT41 values. This behavior is expected with the increase of lattice defects. The scatter in the data documents the natural scatter in the microstructure of similar irradiated material but different specimens and can also be observed in the Charpy test data. Compared with the amplitude dynamic as function of the brittle-to-ductile transition temperature this scatter is smaller than 17%. The influence of an inhomogeneous weld microstructure which was measured with < 4% amplitude variation is much smaller.
Time gate Figure 11. Echo sequence recorded at a Charpy specimen (abscissa time scale, ordinate the electrical voltage which is induced in the EMAT by the ultrasonic wave)
Figure 12. Measuring quantity E60 as function of the shift of the brittle-to-ductile transition temperature dT41 at P16 material
Conclusion Micromagnetic NDT techniques show a high potential when neutron degradation is characterized. The combination and data fusion of micromagnetic measuring quantities in a 3MA-approach is suitable to early detect material degradation. The evaluation of a magnetostrictively transmitted and received ultrasonic wave propagating in the pressure vessel wall thickness direction as a standing wave has special potential to enhance ISI. The two techniques are under development.
References [1] [2] [3] [4]
I. Altpeter, et al., Electromagnetic and Micro-Magnetic Non-Destructive Characterization (NDC) for Material Mechanical Property Determination and Prediction in Steel Industry and in Lifetime Extension Strategies of NPP Steel Components, Inverse Problems 18 (2002) 1907-1921. G. Dobmann, et al., Electromagnetic Characterization of Materials Degradation due to Neutron Irradiation and Fatigue, Applied Electromagnetics and Mechanics (2003), 30-31. G. Dobmann, et al., Aging Material Evaluation and Studies by Non-Destructive Techniques (AMESNDT) - a European Network Project, Nuclear Engineering and Design 26 (2001) 373-374. I. Altpeter, et al., Review of Progress in Quantitative Nondestructive Evaluation. 22A, Melville, New York, American Institute of Physics (AIP) (2003) 15-21.
62
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-62
Evaluation of Chill Contents in Flake Graphite Cast Irons Using AC Magnetization Method Tetsuya UCHIMOTO a,1, Jun MATSUKAWAb, Toshihiko ABEa, Toshiyuki TAKAGIa Takeshi SATOa, Hiroyuki IKEb, Takahito TAKAGAWAc and Noritaka HORIKAWAd a Institute of Fluid Science, Tohoku University, Japan b Graduate School of Engineering, Tohoku University, Japan c Iwate Industrial Research Institute, Japan d Graduate School of Engineering, Hokkaido University, Japan Abstract. In this study feasibility of evaluation for chill contents in flake graphite cast iron is investigated based on AC magnetization method, which is one of the electromagnetic nondestructive evaluation methods. Magnetic properties of flake graphite cast iron samples with different chill contents were measured by a B-H loop analyzer in order to discuss their relation to chill contents. It was found that some magnetic parameters of the flake graphite cast iron depend on the contents of matrices and graphite. Especially, the hardness, which reflects chill contents, has good correlation with the area of hysteresis loop at relatively high frequencies. Focusing on the finding, AC magnetization method was applied to evaluation for the chill contents. Through the experiment, it was found that there is a correlation between hardness of flake graphite cast irons with chill and signals. In consequence, AC magnetization method has a capability of evaluating chill contents in flake graphite cast irons. Keywords. cast iron, AC magnetization method, nondestructive evaluation, chill
1. Introduction In foundry industry, thin-walled mechanical components of cast irons provide weight saving of automobiles, resulting in realization of energy saving vehicle. However, thinwalled components of cast iron leads to the increase in cooling rate during solidification of the cast irons, so that chill, namely proeutectic cementite microstructure, is crystallized. Chill deteriorates the mechanical properties because cast irons including chill are hard and brittle [1]. In contrast, it was reported that chill improves wear resistance, and it can be applied to sliding parts of automobile components such as cylinder bores and piston rings to be endured in severe wear conditions [2]. Therefore, it is highly required in foundry industry to evaluate and 1 Corresponding Author: Institute of Fluid Science, Tohoku University, 2-1-1 Katahira, Aoba, Sendai, Miyagi 980-8577 Japan; E-mail:
[email protected]
T. Uchimoto et al. / Evaluation of Chill Contents in Flake Graphite Cast Irons
63
control chill contents. At present, visual test of fracture surface, microscopic observation and indentation test are applied to evaluate chill contents. However, they are all destructive testing and total inspection is impossible by these methods. For the reason, there is a requirement for establishment of the method to evaluate chill contents nondestructively and quantitatively. Cast iron is composed of graphite and matrices consisting of ferrite, pearlite, chill and so on. Therefore, it is indispensable to extract the information concerned with chill contents from other information including that of graphite and other matrices contents when nondestructive evaluation is applied to estimation of chill contents. Focusing on the difference of electromagnetic properties of each matrix and graphite, some attempts have been done to estimate hardness, other mechanical properties, ratio of ferrite to pearlite in ductile cast iron and graphite size in flake graphite cast iron by the method based on electromagnetic phenomena [3-6]. Feasibility of evaluation for chill contents in ductile cast iron was reported [7]. This work proposes an evaluation method of chill contents by means of the electromagnetic nondestructive method. In this paper, firstly, the contents of matrices and graphite in the flake graphite cast irons with different contents of chill are quantified from the analysis of microstructure. Secondly, the relations between electromagnetic characteristics and the contents of each matrix and graphite are discussed. Finally, focusing on the relation, AC magnetization method is applied to evaluation for chill contents.
2. Cast Metals The flake graphite cast irons which have chemical composition listed in Table 1 were prepared. Materials without chill were divided into three groups: FC150, FC200 and FC250 (JIS standard). In addition, each group has three types of materials depending on three kinds of heat treatments: as cast, furnace cooling and air cooling. In the case of furnace cooling and air cooling, the cast material was reheated at 850 oC in the furnace for one hour. Then, the material was cooled in the furnace or in air, respectively. Therefore, there were 9 materials in the group of the flake graphite cast irons without chill. There were other sets of flake graphite cast iron materials which include chill: I-1 and I-2. They included different contents of chill. The molten metal of cast iron in the group of I-1 and I-2 was same as FC250 and FC150, respectively. In order to obtain chill, following casting process were carried out. Source material, consisting of pig iron, ferrosilicon, electrolytic manganese and electrolytic iron, was melted at 1500 oC. The chemical composition of materials was controlled by retention time of molten metals at 1500 oC. As retention time of the molten metal at 1500 oC increase, CE value, which is defined by 1 CE mass %C ( mass % Si mass % P ) (1) 3 was decreased, and chill was obtained more easily. Chill contents were increased from I-1-1 material to I-1-3 one. It is same on the group of I-2 materials. There was no inoculant into molten metals. Microstructures of the flake graphite cast iron materials were observed by optical microscope to evaluate the size, the shape and the contents of graphite and matrices in
64
T. Uchimoto et al. / Evaluation of Chill Contents in Flake Graphite Cast Irons
them. Pearlite was etched by picric acid ethanol. Some representative photographs are shown in Figure 1. The photos of all materials were analyzed and the areas of each matrix and graphite were quantified. Graphite area was calculated from the photos of the microstructure before etching, and that of matrices was quantified from the picture of microstructure after etching. The contents of graphite and matrices in the materials are summarized in Table 2.
Table 1 Chemical composition of materials. C%
Si%
Mn%
P%
S%
CE%
FC150
3.77
2.78
0.78
0.025
0.015
4.71
FC200
3.36
2.15
0.69
0.018
0.01
4.08
FC250
3.13
1.66
0.72
0.017
0.002
3.69
I-1-1
3.40
1.81
0.66
0.016
0.008
4.01
I-1-2
3.23
1.84
0.66
0.016
0.009
3.85
I-1-3
3.01
1.84
0.66
0.016
0.009
3.63
I-2-1
3.99
2.59
0.77
0.025
0.011
4.86
I-2-2
3.78
2.62
0.77
0.025
0.010
4.66
I-2-3
3.48
2.63
0.76
0.024
0010
4.36
Table 2 Contents of graphite and matrices in each material. Graphite%
Ferrite%
Pearlite%
Chill%
FC150 as cast
11.8
11.3
72.4
0.00
FC150 furnace
13.6
69.3
17.1
0.00
FC150 air
11.1
8.85
71.0
0.00
FC200 as cast
8.25
6.60
85.2
0.00
FC200 furnace
6.45
78.5
15.1
0.00
FC200 air
6.45
4.45
89.1
0.00
FC250 as cast
4.33
3.50
92.2
0.00
FC250 furnace
4.65
40.5
54.9
0.00
FC250 air
4.50
5.20
90.3
0.00
I-1-1
0.45
0.00
68.2
22.9
I-1-2
0.17
0.00
71.5
28.3
I-1-3
0.25
0.00
76.8
31.4
I-2-1
16.4
0.00
75.5
8.1
I-2-2
6.54
0.00
78.5
15.0
I-2-3
1.78
0.00
77.0
21.2
T. Uchimoto et al. / Evaluation of Chill Contents in Flake Graphite Cast Irons
(1)G FC150 as cast sample (before etching)
65
(2)G FC150 as cast sample (after etching)
(3)G I-1-1 sample (before etching) (4)G I-1-1 sample (after etching) Figure. 1 Microstructure in flake graphite cast iron.
3. Magnetic Properties Magnetization curve was measured by the B-H analyzer. The B-H analyzer is composed of pickup coils and an exciting coil. Cylindrical sample is inserted in pickup coil. AC current flowing in an exciting coil generates uniform magnetic field around a sample. Magnetization process in the sample is obtained by a signal of pickup coil. Some parameters such as loop area, remanence and coercivity are calculated from the hysteresis curves obtained by the B-H loop analyzer. The cylindrical samples were processed from the materials. Length and diameter of samples were 30 mm and 3 mm, respectively. Hysteresis curve was measured at the frequencies of 10 Hz and 100 kHz. In the case of 10 Hz, we consider that the measurements are quasi-static, and demagnetizing field correction was made to measured loops. In the case of 100 kHz, no correction was made, which means that the loops should be compared relatively. Figure 2 shows hysteresis curves of some samples at the frequency of 100 Hz. Shape of Magnetization loop depend on the contents of matrices and graphite. Especially, magnetic flux density of the sample without chill at relatively high magnetic field increases with decreasing graphite contents. However, magnetic flux density of I-1-1 sample is relatively small in spite of its low graphite contents. It was found that the sample with chill possesses specific difference from other sample without chill in
T. Uchimoto et al. / Evaluation of Chill Contents in Flake Graphite Cast Irons
/ CIPGVKEHNWZFGPUKV[ )
(% CUAECUV (% CUAECUV (% CUAECUV + +
/ CIPGVKE(KGNF 1 G
Figure 2. B-H characteristics at the frequency of 10Hz.
.QQRCTGC ,O
(% CUECUV (% HWTPCEG (% CKT (% CUECUV (% HWTPCEG (% CKT (% CUECUV (% HWTPCEG
(% CKT + + + + + +
* CTFPGUU* 8
Figure 3. Relation between loop area and hardness at the frequency of 10Hz.
/ CIPGVKEHNWZFGPUKV[ )
66
(% CUAECUV (% CUAECUV (% CUAECUV + +
/ CIPGVKEHKGNF 1 G
Figure 4. B-H characteristics at the frequency of 100 kHz.
T. Uchimoto et al. / Evaluation of Chill Contents in Flake Graphite Cast Irons
67
(% CUAECUV (% CKT (% HWTPCEG + (% CKT + (% CUAECUV + (% HWTPCEG + (% CKT + (% CUAECUV + (% HWTPCEG
.QQRCTGC,O
* CTFPGUU* 8
Figure 5 Relation between loop area and hardness at the frequency of 100kHz.
magnetic characteristics. Hardness of a cast iron mainly depends on both chill and graphite contents. Focusing on the fact, the loop area calculated from hysteresis curve was evaluated as function of hardness of the sample. There is little correlation between the hardness and loop area of each specimen. Figure 4 presents hysteresis curves of the same sample shown in Figure 2 at the frequency of 100 kHz. Shape of magnetization loop is also related to the contents of matrices and graphite. Loop area of hysteresis curve of each sample was also evaluated as function of hardness in Figure 5. In contrast with the relation at 10 Hz, they decreased linearly as hardness increases. The set of samples plotted in Figure 5 includes flake graphite cast iron samples without chill structure, FC150, FC200 and FC250 as well as ones with chill structure. In addition, each series of FC150, FC200 and FC250, which has different graphite shapes, includes samples with different matrices owing to heat treatments. Therefore, hardness of the samples reflects chill contents, graphite shapes and matrices, which implies that loop area at relatively high frequencies depends on chill contents, graphite shapes and matrices. Since there is no correlation between loop area and hardness at low frequency, linear correlation between them at relatively high frequencies is due to effects of eddy currents which depends on permeability and conductivity. Permeability and conductivity of all samples were measured the by BH analyzer and four-terminal method, respectively. Both of them do not have any correlation with hardness. Its mechanism should be complicated since eddy currents flows in heterogeneous media consisting of different types of matrices and graphite structures, which will be discussed in future.
4. AC Magnetization Method Based on the finding acquired from the evaluation of magnetic properties by means of B-H analyzer, AC magnetization method was applied to evaluation for chill contents, and its feasibility was discussed. Schematic drawing of experimental setup is shown in Figure 6. The probe consists of two coaxial pancake coils with a ferrite core; upper coil is an exciting coil, and lower one is a pickup coil. A ferrite core is put to obtain
T. Uchimoto et al. / Evaluation of Chill Contents in Flake Graphite Cast Irons
Function generator
FFT analyzer PC
exciting ferrite exciter detector sample pickup Figure 6 Experimental setup for AC magnetization method.
2 KEMWR 8
(% CUECUV
'ZEKVG 8
Figure 7. Hysteresis equivalent curve at the frequency of 3kHz.
13.0
FC150 as_cast FC150 furnace FC150 air FC200 as_cast FC200 furnace FC200 air FC250 as_cast FC250 furnace
12.5 2
Loop area (V )
68
FC250 air I-1-1 I-1-2 I-1-3 I-2-1 I-2-2 I-2-3
12.0
11.5
11.0
100
200
300
400
500
Hardness HV
Figure 8. Relation between loop area of lissajous and hardness.
T. Uchimoto et al. / Evaluation of Chill Contents in Flake Graphite Cast Irons
69
stronger magnetic field. AC current flowing in exciting coil induces AC magnetic field into a sample. Magnetization process of the sample is detected by the voltage of a pickup coil. Changes of hysteresis curve were easily acquired by plotting lissajous waveform composed of signals of an exciter and a detector (hysteresis curve equivalent), and amplitude of 3rd harmonic wave acquired by a signal of pickup coil. The samples were large enough not to neglect edge effect of them. Outer and inner diameter of exciting coil and pickup one is 8.4 mm and 5.4 mm, height is 4.25 mm and turn number is 150. Applied voltage was 5 V, and measurement was carried out at 3 kHz. Figure 7 shows hysteresis curve equivalent measured from the sample of FC150 as cast. We investigated relationship between the amplitude of 3rd harmonics and hardness. Correlation between them was not confirmed. Figure 8 shows relation between hardness and loop area calculated from the hysteresis curve equivalent obtained from each sample. Tendency of decrease in loop area accompanied with decrease in hardness indicates the feasibility of evaluation of hardness. It is expected that correlation between hardness and loop area improves due to accurate evaluation of loop area accomplished by optimization of the measurement condition.
5. Summary In this paper, dependence of chill contents on magnetic properties was discussed through investigation of magnetic properties of flake graphite cast iron with different chill contents. Based on the insight obtained from the investigation, AC magnetization method was applied to evaluation for chill contents. As the results, it was found that the loop area of hysteresis curve equivalent has correlation with hardness which reflects chill contents, which implies the feasibility of nondestructive evaluation for chill contents by AC magnetization method. Acknowledgements This work is partially supported by New Energy and Industrial Technology Development Organization, Japan, Industrial Technology Research Grant Program, “Characterization of microstructure of advanced cast iron for energy-saving automobile based on multi-scale electro magnetic approach”, 04A48512. The author appreciates many supports by Tsutomu Watanabe and technical staffs in the Institute of the Fluid Science in processing the samples prepared in this study. References [1] [2] [3] [4]
Handbook of foundry engineering (MARUZEN). J.JFS, 2002, 227 T. Nagai, M. Uemura, J. Fujioka, H. Hattori. J.JFS. 2004, 76(6), 440-446 T. Abe, T. Uchimoto, T. Takagi, S. Tada. J.JFS. 2003, 75(10), 675-681 T. Uchimoto, T. Takagi, S. Konoplyuk, T. Abe, H. Huang and M. Kurosawa. Journal of Magnetism and Magnetic Materials, 2003, 1(258-259), 493-496 [5] S. Konoplyuk, T. Abe, T. Uchimoto, T. Takagi, M. Kurosawa, NDT&E International, 2005, 38(2005), 623-626 [6] G. Vértesy, T. Uchimoto, T. Takagi, I. Tomáš, O. Stu-pakov, I. Mészáros, J. Pávó, Physica B, 372(2006), 156-159 [7] M. Kurosawa, T. Uchimoto, T. Abe, T. Takagi, T. Sato, H. Kage, T. Noguchi, J.JFS. 2005, 77(12), 826832
70
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-70
Characterisation of Microstructures in Heat Treated Maraging Steel using Eddy Current and Barkhausen Emission Techniques K.V. Rajkumar, B.P.C. Rao, B. Sasi, S. Vaidyanathan, T. Jayakumar and Baldev Raj Nondestructive Evaluation Division, Indira Gandhi Centre for Atomic Research, Kalpakkam 603102, India; Phone: 91 44 27480232; Fax: 91 44 27480356; email:
[email protected] Abstract. The effects of ageing induced microstructural changes in M250 Maraging steel widely used in aerospace industries are characterized using electromagnetic nondestructive evaluation (NDE) methods. Eddy current and magnetic Barkhausen emission parameters have been studied and the results are compared with hardness, XRD and transmission electron microscopy (TEM). Keywords. Maraging steel, NDE, Eddy current, Barkhausen emission, Microstructure
Introduction Maraging steel is one of the most preferred structural materials for critical application in aerospace industries due to its excellent mechanical properties [1]. The aging behaviour of the maraging steels has been extensively studied [2-6]. M250 maraging steel components are subjected to solution annealing (SA) at 1093 K for 1 h followed by aging at 755 K for 3-10 h. This heat treatment produces the best combination of mechanical properties i.e. ultra high strength coupled with good fracture toughness due to the precipitation of intermetallic phases in low carbon soft martensitic matrix [5-6]. The early aging period comprises of recovery of martensitic structure and hardening due to precipitation of hexagonal Ni3Ti intermetallic precipitates. The intermediate aging duration is characterized by reversion of austenite accompanied by precipitation of hexagonal Fe2Mo intermetallic phase. As these two processes occurring during the intermediate aging drastically affect the hardening in opposite manner, overall hardening levels off after reaching a maximum. Decrease in hardening, observed during longer aging durations is attributed essentially to the formation of reverted austenite rather than the precipitate coarsening. The amount of reverted austenite is reported to increase with increase in aging temperature (upto ~ 900 K) and time [2]. Hence, this regime is of great technological importance. Quantitative characterization of microstructures using particularly, electromagnetic (NDE) methods is of much practical interest. These techniques exploit measurements of changes in
K.V. Rajkumar et al. / Characterisation of Microstructures in Heat Treated Maraging Steel
71
electrical and magnetic properties of materials. Among others eddy current (EC) and magnetic Barkhausen emission (MBE) techniques are preferred, essentially because they are non-contact in nature, sensitive, versatile and field employable. The present study attempts to investigate the effects of aging induced microstructural changes on the eddy current and Barkhausen emission measurements for exploring the possibility of using these methods in shop-floor for verifying the adequacy of heat treatment. Observations of the electromagnetic methods are correlated with hardness, X-ray diffraction (XRD), selected area diffraction (SAD) and transmission electron microscopy (TEM) data.
Figure1. Schematic of experimental setup used for eddy current testing and detailed dimensional drawing of T/R probe.
1. Experimental The chemical composition (wt %) of the maraging (M250) steel used in this study is as follows: 17.89 Ni, 8.16 Co, 4.88 Mo, 0.43 Ti, 0.05 Mn, 0.05 Cr, 0.05 Si, 0.05 Cu, 0.096 Al, 0.003 C, balance Fe. A plate of M250 maraging steel was solution annealed at 1093 K for 1 h followed by air cooling. Specimens of dimensions 30x25x7 mm3 cut from the solution annealed plates, were encapsulated in quartz tubes under vacuum and aged at 755 K for different durations of 0.25, 1, 3, 10, 30, 40, 70 and 100 h followed by water quenching. The eddy current measurements were carried out at 100 kHz using a transmitreceive coil (T/R) type eddy current probe (Figure 1). The EC measurements were carried out after balancing the probe in air and phase angle of induced voltage was adjusted such that the signal of reference stainless steel (SS) 304 specimen was along the positive side of the X-axis [7, 8]. For MBE measurements, the samples were subjected to a continuously varying cyclic magnetic field in an electromagnetic yoke with a period of 10 s. The current from the sweep controller circuit was fed to a bipolar high current generator to generate a symmetrical bipolar triangular field. The applied magnetic field H A was measured at the centre of the yoke using a Hall probe (Walker Scientific) connected to a Gauss meter (MG-50 Walker Scientific). The maximum field was set to 1500 Oe for complete magnetic saturation of the specimen. This corresponds to magnetization field strength (H) of 1,20,000 A m-1. Calibration of HA was made with respect to the current applied
72
K.V. Rajkumar et al. / Characterisation of Microstructures in Heat Treated Maraging Steel
to the yoke. The tangential magnetic field HT was measured near the sample surface. Magnetic Barkhausen emission measurements were performed using an encircling pick up coil (5000 turns). The MBE signal was amplified using a low noise pre-amplifier and a post amplifier (80 dB). The magnetic flux density was measured using a 20 turn coil closely wound on the sample connected to a flux meter (Walker Scientific MF5DP). The output voltage signals for all the magnetic parameters were suitably conditioned for digitization using PC based data acquisition. XRD measurements were carried out for estimation of volume fraction of reverted austenite using MAC Science MXP18 X-ray diffractometer with Cr Kα radiation in the complete angular range of 60-130°. Vicker’s hardness measurements were carried out on these specimens at 10 kg load. Averages of five hardness measurements have been made for each specimen. The maximum scatter in the hardness measurements was found to be ± 5 HV10.
2. Results and Discussion Variation in hardness, volume fraction of reverted austenite and resistivity reported in [3] with aging time are shown in Figure 2. The resistivity curve shows continuous decrease up to 40 h and then leveling off at long aging duration (beyond 40 h). The initial decrease is attributed to the recovery (that includes the removal of quenched in point defect and annihilation of dislocations) in martensite matrix and due to accumulation of solute atoms on dislocations in martensitic matrix. Further decrease in the resistivity and increase in permeability at intermediate durations is attributed to the intermetallics precipitation which is also accompanied by increase in the hardness. The leveling off, observed at longer aging periods (beyond 40 h) is attributed to net manifestation of two opposing mechanisms occurring simultaneously i.e. precipitation and austenitic reversion (decreases hardness).
30
1
10
100
1000
Vol.% of austenite Hardness Resistivity
SA
20
Hardness, HV10
Vol. % of austenite
25
15 10 5
650
0.65
600
0.60
550 500 450
Resitivity (μohm-M)
0.25
35
0.55 0.50 0.45
400
SA
0.40
0 0.25
1 10 Aging time, h
100
350
Figure 2. Variation of hardness, electrical resistivity and volume percent of austenite with aging time (resistivity data is taken from [3]).
Imaginary component of induced voltage, volts
K.V. Rajkumar et al. / Characterisation of Microstructures in Heat Treated Maraging Steel
73
2.5
μr
2.0 Ferrite
SA 0.25h 1h 3hrs 10hrs 30hrs 40hrs 70hrs 100hrs Reference
ρ
1.5 1.0
Carbon steel
0.5 θ
0.0
SS 304
Air
Al 3003
-0.5 -1.0
-0.5
0.0
0.5
1.0
1.5
2.0
ρ 2.5
Real component of induced voltage, Volts
Figure 3. Variation of EC induced voltage in receiver coil with aging time. The complex plane diagram of induced voltage obtained for heat treated maraging steel specimens is shown in Figure 3. The induced voltage is segregated into two distinct clusters marked in square and oval and they are found to be in the second and first quadrant, respectively. The location of these two clusters confirms that the specimens are ferro-magnetic. Cluster in the second quadrant (marked as square) corresponds to ferromagnetic induced voltage of specimens aged up to 10 h and the cluster in the first quadrant (marked as oval) correspond to samples beyond 10 h of aging. Formation of two clusters is essentially due to two distinct microstructural evolution taking place during aging and the associated changes in the resistivity and the permeability. The magnitude and phase angle of the induced voltage are determined and are shown in Figure 4a for various specimens. It can be seen that both magnitude and phase angle are influenced by microstructure changes and their trends are nearly identical. The EC induced voltage is found to increase initially from solution annealed (SA) condition to 0.25 h of aging and then continued to decrease gradually upon aging further up to 10 h. Aging between 10h and 30 h showed a drastic drop in magnitude and phase angle of induced voltage and which continued to drop further gradually in the aging regime of 30-70 h. Beyond 70 h, a drastic drop in induced voltage was noticed. The changes observed in EC parameters can be explained as follows: The initial aging regime (SA-10h) is primarily characterized by dislocation annihilation and precipitation of Ni3Ti intermetallics typically shown in Figure 5a by TEM studies. Annihilation of dislocation is attributed to increase magnetic permeability and reduction in resistivity. Increase in magnetic permeability (associated with dislocation annihilation), as reported by Sablik et al. [9], tries to increase the induced voltage while decrease in resistivity, associated with the precipitation of intermetallics and dislocation
74
K.V. Rajkumar et al. / Characterisation of Microstructures in Heat Treated Maraging Steel
annihilation, tries to decrease the induced voltage. The changes in induced voltage observed for initial aging regime from SA-10 h hence, can be understood in terms of net manifestation of two opposing mechanisms i.e. dislocation annihilation and intermetallic precipitation. The larger decrease in EC parameters for specimens aged to 30h is attributed to initiation of non-magnetic reverted austenite in addition to the continuous precipitation of intermetallics (Ni3Ti and Fe2Mo). Non-magnetic austenite phase lowers the overall permeability and simultaneous precipitation of intermetallics decreases the resistivity, both contributing to drastic decrease in EC parameters. The presence of reverted austenite has been reported detrimental to toughness due to the deformation concentration at softer austenite, which reaches its critical strain of fracture at early stage. Hence, the microstructures containing austenite are avoided and this can be ascertained by using either of the EC parameters with appropriate thresholds. The regime of technological importance (3h-10h) can also be identified by specifying the corresponding EC parameters as they exhibit monotonous decrease in this regime in Figure 4a. Between 30h and 70h, the EC induced voltage again changed very gradually showing that the microstructural feature changes occurring do not influence the EC induced voltage substantially. This is attributed to subtle increase in the volume fraction of reverted austenite formed along with the precipitation, as evident from austenite and hardness measurements in Figure 2. For the aging regime 70-100 h, since the resistivity values Figure 2 remain almost constant, the observed drastic decrease in the EC parameters is attributed to larger reduction in overall permeability due to larger volume fraction of reverted austenite as evident from the XRD results in Figure 2. This study reveals that both magnitude and phase angle of induced voltage can be used as NDE parameters for characterization of the microstructures of M250 steel. Further, time for each measurement is less than 1 second. As compared to phase angle, measurement of magnitude of induced voltage is accurate and easy. It is also easy to implement the EC method in production line using portable eddy current instruments and probes. Thus, this method holds a great promise for quick and reliable characterization of microstructures in components in shop-floor for ensuring heat treatment adequacy. 2.4
1
10
100 EC phase EC magnitude
SA SA
100
2.5
96
2.0
92
88
1.8 84
EC phase angle (θ)
EC magnitude (V)
2.2
2.0
0.25
1
10
100
1
10
100
SA
MBE rms voltage, V
0.25
1.5
1.0
0.5
1.6 0.25
1
10
Aging Time, h
100
80
0.0
0.25
Aging time, h
(a) (b) Figure 4. (a) Variation of induced voltage magnitude and phase angle with aging time and (b) variation in rms voltage of MBE signal with aging time.
K.V. Rajkumar et al. / Characterisation of Microstructures in Heat Treated Maraging Steel
75
(A)
(B) (C)
0.5 μm (a)
0.5 μm (b)
Figure 5. (a) Bright field TEM image of specimen solution annealed at 1093 K for 1 h followed by air cooling (showing high dislocation density) (b) Bright field image of the specimen thermally aged at 755 K for 100 h followed by water quenching, showing long and patchy austenite (marked as A), patchy Ni3(Ti, Mo) (marked as B) and globular Fe2Mo (marked as C). The MBE rms peak voltage was found to vary with aging time as typically shown in Figure 4b and the MBE trends were almost identical to eddy current measurements. The MBE rms peak voltage remained almost constant from solution annealed condition to 10 h of aging and dropped drastically on further aging. The solution annealed microstructure is characterized by the martensitic lath/grain boundaries. In this condition, the magnetic domains have to cross several martensitic lath/grain boundaries before they give a detectable signal at the sensor coil. The constant MBE rms peak voltage obtained from SA condition to 10 h of aging can be attributed to the two opposing mechanisms taking place simultaneously i.e. dislocation annihilation and intermetallic precipitation. Martensitic recovery, due to the annihilation of dislocations occurring during initial aging is expected to increase the MBE by reducing the number of pinning sites for domain wall motion. However, this regime is also characterized by the continuous precipitation of intermetallics. Aging in this regime results in increase in the precipitates which act as strong pinning sites to domain wall motion, thereby reduction in MBE rms peak voltage is expected. The drastic decrease in MBE rms peak voltage beyond 10 h of aging is attributed to the initiation of the reversion of non-magnetic austenite phase. It is evident from the TEM studies that austenite is formed at martensitic lath /grain boundaries. The austenite formed at these lath and grain boundaries make these region nonmagnetic, which cannot be easily surmounted by the growing/moving magnetic domains. Moreover, the non-magnetic austenite phase is expected to be surrounded by stable closure domains. Under these conditions, magnetization reversal can only advance in
76
K.V. Rajkumar et al. / Characterisation of Microstructures in Heat Treated Maraging Steel
limited volume fraction of the specimen at any given instant and the actual fraction depends on the amount of reverted austenite. Aging for longer durations results in increase in the volume fraction of the austenite, which further decreases the MBE rms peak voltage. The evidence for increase in austenite volume percent is obtained from XRD analysis (Figure 2) and TEM studies (Figure 5b). Hardness and magnetic parameters exhibited different behaviour upon aging. Hardness increased with the precipitation of intermetallic phases and decreased with the reversion of austenite. The MBE rms peak voltage was found to be highly sensitive to austenite reversion and was however insensitive to intermetallics precipitation during aging. Hardness was found to be influenced more by the intermetallic precipitates as compared to austenitic phase reversion. The reversion of austenite at 30 h of aging could not be identified by the hardness due to simultaneous precipitation of intermetallics, which tend to increase the hardness. The regime of technological importance 3-10 h could not be identified by hardness or MBE parameter alone. However, the study clearly revealed that the combination of these two parameters, i.e. by specifying a minimum hardness (564 VHN) and a minimum MBE rms peak voltage (1.8V) can be used for unambiguous characterization of the microstructure of technological importance in M250 maraging steel [10].
3. Conclusion The present study investigated the influence of microstructural features evolved upon aging of M250 maraging steel at 755 K for different durations on electromagnetic NDE (eddy current and MBE) parameters. In eddy current method both magnitude and phase angle of induced voltage of receiver coil were found to be sensitive to the microstructure changes through electrical conductivity and magnetic permeability. The EC parameters could distinctly identify the over-aging due to austenite reversion, a non-magnetic phase in magnetic matrix. The dislocation annihilation and intermetallics precipitation were also found to influence the EC parameters. For the first time, it has been observed that using EC parameters it is possible to study the recovery (i.e. removal of quenched-in point defect and annihilation of dislocations) during initial aging which increases the magnetic permeability and decreases resistivity. The monotonous decrease in EC parameters can be effectively used to identify the aging regime of technological importance (3-10h) at 755 K. The MBE rms peak voltage was also found to be highly sensitive to austenite reversion and was however insensitive to intermetallics precipitation during aging. Hardness was found to be influenced more by the intermetallic precipitates as compared to the austenitic phase reversion. The reversion of austenite at 30 h of aging could not be identified by the hardness due to simultaneous precipitation of intermetallics, which tend to increase the hardness. The regime of technological importance 3-10 h could not be identified by hardness or MBE parameter alone. However, the study clearly revealed that the combination of these two parameters can be used for unambiguous characterization of the microstructure of technological importance in M250 maraging steel. The study also established that electromagnetic non destructive methods hold good promise for shop floor assessment of heat treatment adequacy.
K.V. Rajkumar et al. / Characterisation of Microstructures in Heat Treated Maraging Steel
77
Acknowledgements Authors thank Dr. P. Shankar, Dr. Anish Kumar and Mr. S. Mahadevan of Indira Gandhi Centre for Atomic Research (IGCAR), Kalpakkam, India for many useful discussions. References [1] [2] [3] [4] [5]
G.P. Miller, W.I. Mitchell, J. Iron Steel Inst. 203 (1965) 899-904. D.T. Peters, C.R. Cupp, Trans. Met. Soc. AIME 236 (1966) 1420-1429. V.K. Vasudevan, S.J. Kim, C.M. Wayman, Metall. Trans. A 21, (1990) 2655-2668. W. Sha, A. Cerezo, G.D.W. Smith, Metall. Trans. A 24 (1993) 1221-1232. R.F. Decker, S. Floreen, IN: R.K. Wilson (Ed.), Maraging Steels: Recent Developments and Applications, TMS-AIME, Warrendale, PA, (1988) 1–38. [6] Z. Guo, W. Sha, D. Vaumousse, Acta Mater. 51 (2003) 101-116. [7] B.P.C. Rao, Introduction to eddy current testing, Narosa Publishing, New Delhi, April, 2007 [8] K.V.Rajkumar, B.P.C. Rao, B.Sasi, Anish Kumar, T.Jayakumar, Baldev Raj and K.K. Ray, Materials Science and Engg. A 464 (2007) 233-240. [9] M.J. Sablik, J. of Appl. Phys. 89 (10) (2001) 5610-5613. [10] K.V. Rajkumar, S. Vaidyanathan, Anish Kumar, T. Jayakumar, Baldev Raj and K.K. Ray, J. of magnetism and magnetic materials 312 (2007) 359-365.
78
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-78
Novel Acoustic Barkhausen Noise Transducer and its Comparison with Electromagnetic Acoustic Transducer John WILSON1, Gui Yun TIAN1, Rachel S. EDWARDS2 and Steve DIXON2 School of Electrical, Electronic and Computer Engineering, Newcastle University, NE1 7RU, 2Department of Physics, University of Warwick, Coventry, CV4 7AL
1
Abstract
The analysis of magnetic Barkhausen noise (MBN) has been used to provide information about the stress state and microstructural properties of ferromagnetic materials. Recent work has shown that a technique using acoustic Barkhausen noise (ABN) detection can provide the similar capabilities as traditional MBN along with additional information for defect characterisation and thickness measurement in a single system. Because the detection of ABN using a piezoelectric sensor can be carried out at any point on the material surface, as well as analysing ABN for microstructural characterisation, the interaction of the surface propagating waves with defects can also be analysed and used for defect characterisation, along with frequency analysis for thickness measurement. As with electromagnetic acoustic transducer (EMAT) systems, the ABN technique applies totally different physical principles to traditional ultrasonic methods and couplant is not needed for excitation. The work is carried out through experimental investigations of calibrated steel samples with machined defects using the ABN system, in comparison to readings taken using an EMAT system. Test results show that the ABN technique has potential applications in providing a comprehensive system for material and stress characterisation along with the additional capabilities of defect characterisation and material thickness measurement.
Introduction The inspection of ferromagnetic structures such as oil and gas pipeline [1], rail track [2] or ferromagnetic components in manufacturing is a common requirement in industry, and there is wide need for accurate defect detection and characterisation apparatus for the prediction of failure in ferromagnetic engineering structures and components. This is to some degree addressed by current inspection techniques, but each method has drawbacks, for example magnetic flux leakage (MFL) has good detection capabilities, but there is difficulty in extracting accurate characterisation data [1], although the recently introduced pulsed MFL (PMFL) system has improved the potential capabilities of MFL [3]. A reasonable standard of detection and characterisation can be achieved with ultrasonic testing [2, 4-12], but with some limitations for standard contact ultrasonic measurements. This has led to the development of alternative non-contact excitation techniques.
J. Wilson et al. / Novel Acoustic Barkhausen Noise Transducer
79
Acoustic sources for ultrasonic NDE fall into two categories: contact techniques requiring direct acoustic coupling between the source and the material under inspection, and non-contact techniques. The major drawback of contact transducers is the need to provide acoustic coupling between the element and the material under inspection, so real world inspections usually require extensive surface preparation and removal of coatings adding to time and expense. There are clear advantages in techniques where physical contact between transducer and the area under inspection is not required. Techniques used to address the problem include guided wave technology [4], where the sensors are located remotely to the area under inspection, water coupled systems [5, 6], where the material and transducer are immersed in a water tank, pulsed laser generation of ultrasonic sources [7, 8] and air coupled systems [9,10]. The major drawback of an air-coupled system is the miss-match in acoustic impedance between air and solid materials [9], meaning that overall path losses for an air coupled system can be 100dB + higher than water coupling, with the greatest losses occurring with ferrous metals [10]. In contrast to other non-contact techniques, electromagnetic acoustic generation opens up opportunities for ultrasonic generation without direct access to the material surface [11]. As coupling between transducer and material is provided electromagnetically, inspection through coatings and corrosion layers is possible and coupling can be established to materials with irregular surface geometry. The most commonly used electromagnetic ultrasonic source is the electromagnetic acoustic transducer (EMAT) [2, 11, 12]. EMAT transducers consist of an excitation coil driven by a current pulse in the presence of a static magnetic field. In non-magnetic conductive materials such as aluminium, application of a current pulse to the coil in presence of the permanent field causes Lorentz forces in the material, which in turn generate acoustic waves. In magnetic and conductive materials such as steel, magnetostrictive effects occur in addition to Lorentz forces. Although EMATs provide a solution to the coupling problem in electrically conductive and magnetic materials, the ultrasonic generation efficiency of an EMAT is much lower than that of a piezoelectric transducer. In this paper, a new electromagnetically generated acoustic source for ferromagnetic materials is proposed utilising acoustic Barkhausen noise (ABN). As well as providing a non-contact excitation method for ultrasonic investigation, ABN uniquely carries information about the stress and microstructure of the material within the signal itself. The technique has the potential to provide an affordable, low power, non-contact solution for electromagnetically induced acoustic defect assessment with the potential to also supply stress and material characterisation data.
1. Experimental Investigation of ABN for Acoustic Source Generation When a time varying magnetic field is applied to a ferromagnetic material, the induced magnetism is not continuous; rather, it is made up of jumps in magnetisation corresponding to domain wall movement, this can be detected by a pick-up coil or magnetic field sensor and is known as magnetic Barkhausen noise (MBN) [13]. This domain wall motion also causes a release of elastic energy which manifests itself as an acoustic pulse and can be measured using a piezoelectric sensor; this is known as magneto-acoustic emission (MAE) [14] or ABN [15]. As magnetic domain structure is
80
J. Wilson et al. / Novel Acoustic Barkhausen Noise Transducer
intrinsically linked material microstructure, MBN and ABN are sensitive to material stresses and changes in microstructure [13-15]. This work extends ABN beyond microstructure and stress characterisation to provide defect assessment capabilities using broadband excitation. In contrast to EMATs and most other excitation techniques, the frequency of the measured signal is dependant, not on excitation frequency, but on the frequency of the elastic energy released by domain wall movement. Low frequency excitation can be used, thus dramatically reducing the comparative power consumption of the system.
(a)
(b)
Figure 1: a) Probe design, b) One repetition of positive half cycle of pulsed ABN and excitation signal, with calculated signal profile
The experimental probe is shown in figure 1a. A ferrite core is mounted on the sample under inspection. A piezoelectric sensor is mounted on the material surface with petroleum jelly used to provide acoustic coupling between the sensor and the material. Pulsed excitation is applied to the ferrite core and data acquired from the sensor and the excitation current simultaneously at a sample frequency of 2MHz. In this work, a piezoelectric Physical Acoustics R15I-AST integral preamplifier acoustic emission receiver is used; the sensor is resonant at 150kHz, with a useable frequency range of around 50kHz – 200kHz and a total gain of 72dB is applied to the signal. Figure 1b shows one repetition of the positive half cycle of the pulsed excitation waveform and the associated ABN signal. Several signal processing techniques are used in the work; the most basic of these is calculation of the signal profile or envelope by rectification followed by a moving average calculation as shown in figure 1b. 1.1. Characterisation of ABN signal In an ultrasonic defect detection system, the minimum detectable defect depth is proportional to the wavelength of the signal being measured, so knowledge of the frequency range of the acoustic source is vital for the developed system, but the frequency spectrum of ABN has not been widely studied. Figures 2a and 2b show FFT envelopes for two different materials; a 60mm x 60mm x 1000mm steel block and a 1mm thick mild steel sheet. Sine wave excitation was used in the test, with the ABN signal from six different frequencies from 2Hz to 1kHz recorded for comparison. It can be seen from the plots that the basic distribution of frequency components remains the
81
J. Wilson et al. / Novel Acoustic Barkhausen Noise Transducer
same regardless of excitation frequency, although there is a change in amplitude over the excitation frequencies used. This is as expected, as the frequency spectrum of ABN is dependant on the frequency of the elastic wave released by the motion of the domain wall, not the excitation frequency. FFT ENVELOPES: SINE EXCITATION, STEEL PLATE -2 10
5Hz Excitation 10Hz Excitation 50Hz Excitation 100Hz Excitation 1kHz Excitation
-4
10
-5
10
2Hz Excitation 5Hz Excitation 10Hz Excitation 50Hz Excitation 100Hz Excitation 1kHz Excitation
-3
10 Amplitude(Log)
Amplitude(Log)
FFT ENVELOPES: SINE EXCITATION, STEEL BLOCK -3 10 2Hz Excitation
-4
10
-5
10
-6
-6
10
0
100
200 300 Frequency - kHz
400
10
500
(a)
0
100
200 300 Frequency - kHz
400
500
(b)
(c) Figure 2: ABN frequency spectrum for; a) thin steel plate, b) large steel block, c) ABN amplitude for frequency variation
Comparison of figures 2a and 2b show that, although material properties will certainly play a part in the ABN frequency response, for these unstressed samples, material dimensions have a much greater influence on the frequency spectrum of the induced signal than excitation frequency. With the thicker sample, the lower frequency portion of the signal is enhanced. This is due to the reinforcement of frequency components with wavelengths corresponding to the material dimensions. So at an estimated signal velocity of 3000 m/s, with the 60mm sample the frequency component corresponding to a wavelength of 60mm is 3000 / 0.06 m = 50 kHz and the frequency component corresponding to half the wavelength is 100 kHz. It can be seen from the plot that these areas of the plot are indeed enhanced for the thicker sample. For the thinner sample, the frequency component corresponding to a wavelength of 1mm is 3000 / 0.001 m = 3 MHz, well out of the measured range, so the plot for this sample is much smoother, without the reinforcement of wavelengths corresponding to the thickness of the sample. ABN RMS amplitudes for the frequencies used in the tests are shown in figure 2c. It can be seen from the plot that the ABN amplitude increases as the excitation
82
J. Wilson et al. / Novel Acoustic Barkhausen Noise Transducer
frequency increases. This is due to increasing overlapping of clustered random event outputs as the excitation frequency increases [16]. This increase in ABN amplitude will not continue indefinitely as frequency increases, rather the rate will decrease as the skin-depth effect becomes apparent [16].
2. Application of ABN to defect detection An experiment was set up to assess the capabilities of the system to provide depth information for perpendicular defects in steel. Two samples, shown in figure 3a and 3b, were used, measuring 60mm x 60mm x 600mm (sample 1) and 60mm x 60mm x 1000mm (sample 2). The blocks, contain five 1mm wide defects, with depths of 0.5mm, 2mm, 2.5mm, 3.5mm and 10mm. The test set-up is shown in figure 3c. In these tests a single sensor is used at different distances (d) with respect to slot position, with excitation apparatus kept at a constant distance to the slot. d is given as the distance between the sensor rim closest to the slot and the slot under inspection, at no time in the tests is the sensor actually over the slot. The peak signal strengths for sensor positions from d = 10 to d = -10 are shown in figure 3e. It can be seen from figure 3e that the peak amplitude for all but the 2mm slot shows a maximum at d = 0 or d = 1. The EMAT normalised signal amplitude on approaching a 3mm deep slot in a steel sample is shown in figure 3f [11]. A signal enhancement is also observable in EMAT systems close to material voids where reflections and mode conversions from the slot interfere with the direct signal, as shown in figure 3f [11]. The proportion of transmitted surface wave energy will depend on the crack depth and the wavelengths within the broadband signal, through the transmission coefficients [12]. FFTs were calculated from the AE sensor signals, for four slot depths, and the mean frequencies calculated, as shown in figure 3d. It can be seen from the plot that for the 2.5mm, 3.5mm and 10mm slots the mean frequency decreases in a fairly linearly as the slot depth increases. This indicates that as slot depth increases, more of the lower frequency signal component is reflected back to the sensor. As defect depth increases, the wavelengths which can be reflected by the defect increase, thus lowering the mean frequency of the reflected wave. As the capabilities of an ultrasonic system with respect to measurable slot depth are dependant on the frequency range of the system, it may be that characterisation of the 2mm slot is beyond the capabilities of the ABN system using this particular sensor. With ultrasonic measurements using a wideband Rayleigh wave pulse, the calculated cut-off frequency of the measured signal has been shown to be proportional to slot depth [12].
(a)
(b)
83
J. Wilson et al. / Novel Acoustic Barkhausen Noise Transducer
Frequency - kHz
ABN MEAN FREQUENCY FOR FOUR SLOTS 121.2
121
120.8
120.6
120.4 2
4
6 8 Slot depth - mm
1.3 1.2 1.1 1 0.9 -10
-5 0 5 10 Sensor position with respect to slot - mm
(e)
(d) Normalised signal amplitude
Amplitude - V
(c) ABN PEAK AMPLITUDE OVER DEFECT AREA 2mm SLOT 2.5mm SLOT 1.6 3.5mm SLOT 1.5 10mm SLOT 1.4
10
1.6 1.4 1.2 1.0 0.8 0.6 0.4 -80
-60
-40
-20
0
20
40
Scale (mm)
(f)
Figure 3: a) Test sample 1, b) Test sample 2, c) Defect location test set up, d) Mean ABN frequency for four slot depths, e) ABN peak amplitude over slot area, f) EMAT amplitude approaching a 3mm deep slot in a steel sample
3. Discussion and Conclusions Several parameters, summarised in figure 4, influence the form of the ABN signal, with the greatest influences coming from material properties, sample geometry and excitation waveform. The peak position of the ABN signal with respect to the excitation cycle is influenced by the excitation signal itself and the domain structure of the material, which affects the domain wall activity at different stages in the hysteresis cycle. By far the greatest influence on ABN frequency spectrum comes from the geometry of the sample, through internal reflections of the acoustic signal, but the domain structure will also have some influence through the types of domain wall which are active in the sample. The overall ABN amplitude is influenced by all three parameters, through the amount of domain activity in the sample, reinforcement of the signal through sample geometry and magnetic field intensity in the sample through the amplitude of the excitation signal. The decay of the ABN signal is greatly influenced by sample geometry through reflections received by the sensor after the main domain wall activity has ceased. ABN peak amplitude is of course affected by the overall amplitude of the ABN signal, but also by the excitation waveform. The higher the rate of change of the signal, the more ABN activity will be contained within the same time period, leading to overlapping of acoustic events.
84
J. Wilson et al. / Novel Acoustic Barkhausen Noise Transducer
Figure 4: Contribution of various factors to ABN signal characteristics
ABN can work as an acoustic source which also carries information on material properties, which is a distinct advantage over current acoustic NDT. Although preliminary test results show that ABN has some promise as an acoustic source, there are several problems with technique; the ABN signal intensity is relatively weak; the signal frequency spectrum is dependent on the frequency of elastic energy from domain wall, not excitation frequency – this could be a problem due lack of controllability, but also means that low frequency excitation tuned to the optimal frequency for maximum power transfer can be used to excite high frequency ABN source; unlike the ultrasonic measurements using EMATs, the mode of propagation of the signal is not fully understood; the ABN signal is made up of many different acoustic events – this could be problematic for processing. A piezoelectric sensor is used for present tests, but for true non-contact operation, a non-contact ABN receiver should be developed. Future tests will be made with “real world” defects such as cracks, voids and dislocations and the limitations of the system ascertained. Although the technique will have limitations in terms of the interaction between the wavelength of the excited signal and defect depth, the change in the ABN signal caused by the interaction between domain walls and defects will be incorporated into future measurements.
References [1]
[2]
[3] [4]
[5]
A.A. Carvalho, J.M.A. Rebello, L.V.S. Sagrilo, C.S. Camerini and I.V.J. Miranda, MFL signals and artificial neural networks applied to detection and classification of pipe weld defects, NDT & E International, Volume 39, Issue 8, December 2006, Pages 661-667. Y. Fan, S. Dixon, R.S. Edwards and X. Jian, Ultrasonic surface wave propagation and interaction with surface defects on rail track head, NDT & E International, Volume 40, Issue 6, September 2007, Pages 471-477. J.W. Wilson and G.Y. Tian, Pulsed electromagnetic methods for defect detection and characterisation, NDT & E International, Volume 40, Issue 4, June 2007, Pages 275-283. A. Demma, P. Cawley, M. Lowe, A. G. Roosenbrand and B. Pavlakovic, The reflection of guided waves from notches in pipes: a guide for interpreting corrosion measurements, NDT & E International, Volume 37, Issue 3, April 2004, Pages 167-180. X. Jian, J.P. Weight and K.T.V. Grattan, Miniature wideband ultrasonic transducers to measure compression and shear waves in solid, Sensors and Actuators A: Physical, Volume 127, Issue 1, 28 February 2006, Pages 13-23.
J. Wilson et al. / Novel Acoustic Barkhausen Noise Transducer
[6] [7] [8]
[9] [10] [11] [12] [13]
[14] [15] [16]
85
R.E. Green, Non-contact ultrasonic techniques, Ultrasonics, Volume 42, Issues 1-9, April 2004, Pages 9-16. B.B. Djordjevic, D. Cerniglia, and C. Cosenza, Guided wave non-contact ultrasonic for NDE, WCNDT 2004. Y. Hong, S.D. Sharples, M. Clark and M.G. Somekh, Rapid and accurate analysis of surface and pseudo-surface waves using adaptive laser ultrasound techniques, Ultrasonics, Volume 42, Issues 19, April 2004, Pages 515-518. E. Blomme, D. Bulcaen and F. Declercq, Air-coupled ultrasonic NDE: experiments in the frequency range 750 kHz–2 MHz, NDT & E International, Volume 35, Issue 7, October 2002, Pages 417-426. J. Buckley, Air-coupled Ultrasound - A Millennial Review, WCNDT 2000. R.S. Edwards, A. Sophian, S. Dixon, G.Y. Tian and X. Jian, Dual EMAT and PEC non-contact probe: applications to defect testing, NDT & E International, Volume 39, Issue 1, January 2006, Pages 45-52. R.S. Edwards, S. Dixon and X. Jian, Depth gauging of defects using low frequency wideband Rayleigh waves, Ultrasonics, Volume 44, Issue 1, January 2006, Pages 93-98. V. Moorthy, B.A. Shaw and P. Hopkins, Surface and subsurface stress evaluation in case-carburised steel using high and low frequency magnetic barkhausen emission measurements, Journal of Magnetism and Magnetic Materials, Vol. 299(2), Apr. 2006, pp. 362-375. D. O'Sullivan, M. Cotterell, D.A. Tanner and I. Mészáros, Characterisation of ferritic stainless steel by Barkhausen techniques, NDT & E International, Volume 37, Issue 6, September 2004, Pages 489-496. G.Y. Tian, J. Wilson and J. Keprt, Magnetic-acoustic Emission for Stress and Material Characterisation, ENDE 2006. H.C. Kim and C.G. Kim, Effect of magnetising frequency and stress on magneto-acoustic emission from 3% Si-Fe crystals, Journal of Physics D: Applied Physics, Volume 22, Issue 1, pp. 192-198 (1989).
86
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-86
Modelling and Measurement of Decarburisation of Steels Using a Multifrequency Electromagnetic Sensor X.J. HAOa,1 , W. YINb, M. STRANGWOODa, A.J. PEYTONb, P.F. MORRISc and C.L. DAVISa a Department of Metallurgy and Materials, University of Birmingham, Birmingham, B15 2TT, UK b School of Engineering, University of Manchester, Manchester, M60 1QD, UK c Corus plc. Swinden Technology Centre, Moorgate, Rotherham, S60 3AR, UK
Abstract. Decarburisation of high carbon steel has been simulated, using composite samples comprised of a 316 stainless steel (paramagnetic) core and a surrounding tube of ferritic steel (ferromagnetic) with thicknesses between 100 and 600 μm, for determining the potential for on-line measurement during steel processing. Decarburization samples have also been generated, for off-line measurements, by heat treatment of an Fe-0.8 wt% C steel for various times in air at 1000 – 1200°C. A multi-frequency (10 – 106 Hz) electromagnetic sensor was used to determine variations in inductance (due to differences in permeability) as a function of decarburisation depth. The relationship between sensor output and decarburised layer type/thickness has been modelled using finite element software.
1. Introduction The heat treatment and hot processing of steel usually requires the material to be heated into the austenite phase field, in the temperature range of 800~1200oC. At these temperatures, carbon at the surface can be removed by reaction with oxygen in the surrounding atmosphere and this process is known as decarburisation. Loss of carbon from the surface is more rapid than replenishment by solid-state diffusion, causing a gradient in carbon level from bulk to surface. This effect is greater in higher carbon steels. Loss of carbon at the surface can have a significantly detrimental effect on mechanical properties of products, since hardness, fatigue, strength, and wear properties are strongly dependent on carbon content. Commercially the depth and extent of decarburisation is controlled, which needs accurate measurement of this phenomenon. Currently, measurement of decarburisation is by destructive methods, such as metallographic observation or hardness tests on a cross section of samples after processing. These methods are time consuming and cannot be applied during the production process. This study aims to develop a multi-frequency electromagnetic (EM) sensor to monitor the decarburizing process on-line, and to measure decarburisation depth off-line. Below the Curie temperature (§ 770°C for carbon steel) austenite is paramagnetic and ferrite is ferromagnetic. EM sensors work on the basis of 1
Corresponding author: X.J. Hao, E-mail:
[email protected]
X.J. Hao et al. / Modelling and Measurement of Decarburisation of Steels
87
detecting the difference in relative permeability, μR, and conductivity, V, between microstructural phases or due to changes with temperature. An air cored multifrequency EM sensor can measure the ferrite fraction in steel over the entire ferrite fraction range: from 0-40% ferrite fraction through low frequency inductance; and from 40-100% ferrite fraction through the zero crossing frequency, by the differences in effective permeability of the dual phase microstructure [1,2]. Decarburising at high temperature induces a carbon gradient from surface to interior. During cooling from austenite, the surface layer, with low carbon content, transforms first to ferrite whilst the interior transforms to pearlite later. An EM sensor should therefore be able to measure the decarburisation depth by detecting the ferrite fraction gradient. For on-line measurement, if the EM sensor is placed above the steel when it is between the Curie and eutectoid temperatures, any ferromagnetic ferrite surface layer may be detected compared to the paramagnetic austenite core. For off-line measurements differences in permeability between ferrite and pearlite, which are much less than between ferrite and austenite, would need to be detected.
2. Experimental On-line measurement has been simulated using composite samples comprised of a 316 stainless steel (austenite, paramagnetic) core and a surrounding tube of ferritic steel (0.17 wt% C, ferromagnetic). 316 stainless steel bars, 8mm diameter, were inserted into the ferritic steel tubes (8mm inner diameter, 1mm wall thickness) and then cold drawn to 6.7mm (composite bar outer diameter) to increase contact between core and outer layer. The composite bars (300mm length) were straightened and center-less ground to get ferritic layers with thicknesses of about 100, 200, 300 and 600 μm. For off-line measurements, decarburisation samples were generated, by heat treatment of Fe-0.8 wt% C steel bars (10mm diameter, 150mm length) in an air furnace at 1000°C for various times (10min to 5 hours) then cooled in air. Any loose surface oxidation layer was removed by gentle tapping. Transverse microstructures from each sample were examined by optical microscopy after sectioning, polishing and etching using 2% nital. A multi-frequency electromagnetic (EM) sensor was used to determine variations in inductance (due to differences in permeability) as a function of decarburisation depth. Samples were measured by inserting them into the air-cored cylindrical sensor, which had a length of 10mm and diameter of 20mm and was driven using an impedance analyser at frequencies from 10 to 106 Hz. The relationship between sensor output and decarburised layer type / thickness was modelled by finite element method (FEM) using COMSOL Multiphysics [3] software. Sensor 3. Results and discussion
Austenite Hot on-line testing was simulated using the composite bar samples. Microstructure Ferrite: observation of the composite bars has confirmed that the ferrite layer makes good contact with the austenite. The setup for sensor measurement is Figure 1. Setup of sensor/sample shown in Fig. 1, which was used to model the for experiments and modelling
88
X.J. Hao et al. / Modelling and Measurement of Decarburisation of Steels
sensor output with decarburisation depth. -4
10
a
Inductance (H)
8 6 4 2
b
Frequency: 100Hz
1.0
Ferrite layer thickness (Pm) 0 100 200 300 600
10
Normalized Inductance
12
0.8 0.6
Pr
0.4
50 200 1000
0.2
measured
0 -2 1 10
0.0 2
10
3
10
4
10
Frequency (Hz)
5
10
0
6
100
10
200
300
400
500
600
Decarb thickness (Pm)
Figure 2. (a) Measured inductance vs. frequency for composite bars and (b) comparison between measured and modelled results. 5.0
a
10
-4
b
4.8 4.6
Inductance (H)
4.4 4.2 4.0 3.8 3.6 3.4
200Pm
o
At 1000 C for: 10min Increasing 1hr decarburisation 2hrs 5hrs
3.2 3.0 1 10
2
Frequency
10
Figure 3. (a) Microstructure of Fe-0.8wt%C steel after decarburising at 1000C for 2 hours showing surface ferrite (white) and pearlite (black), and (b) measured inductance change with frequency for samples after various decarburising times at 1000°C. The EM sensor output, in terms of inductance versus frequency is shown in Fig. 2(a). The magnetic field produced by an EM sensor acts on a ferromagnetic target in two ways. First it tends to magnetise the metal, which increases the coil’s inductance. Second, the alternating current magnetic field also induces eddy currents in the metal, which tend to oppose the driving current and reduce the coil’s inductance. At low frequencies, magnetisation dominates the inductance. As the frequency is increased, the effects of eddy current become more dominant and the inductance decreases, eventually approaching a constant value at high frequencies. As shown in Fig. 2(a), the inductance value increases with increasing decarburisation thickness (ferrite layer thickness) at low frequencies. This indicates that the low frequency inductance value is a good parameter for measuring decarburisation thickness. Therefore, the measured and modelled inductance values (normalized for the sample before centre-less grinding, 600μm decarburisation depth, for comparison) at low frequency (100 Hz) versus decarburisation thickness are shown in Fig. 2(b). As the relative permeability of ferrite could not be experimentally determined (and varies considerably with carbon content), three values over a large range (50, 200 and 1000) have been chosen for FEM modelling. Both the measured and modelled results show that inductance changes with decarburisation thickness in a non-linear manner. With increasing decarburisation thickness from zero, the inductance increases quickly, and then tends towards saturation. This phenomenon is due to the demagnetising field effect. When a finite size ferromagnetic sample is magnetised in an applied magnetic field, a demagnetising field appears in the sample, which is opposite to the applied field. For the sample with
X.J. Hao et al. / Modelling and Measurement of Decarburisation of Steels
89
the largest relative permeability (1000), the demagnetising field effect is the most significant. It should be noted that the measured and modelled results are not in perfect agreement. This may be due to non-uniformity of ferrite layer thickness along the rod after grinding, and / or the plastic deformation introduced in the ferrite layer, which affects its permeability [4]. The simulation of on-line testing has shown that the EM sensor has the ability to detect decarburisation depth based on the fact that the relative permeability of ferrite is hundreds of times larger than that of austenite. For off-line testing, the sensor needs to be able to distinguish between the surface ferrite and core pearlite. The relative permeability ratio of ferrite/pearlite is much smaller than ferrite/austenite because pearlite is also a ferromagnetic phase. Thompson and Tanner [5] have shown that the initial relative permeability of pearlite (0.87 wt% C) is 56, whereas ferrite with a small amount of pearlite (0.17 wt% C) is 280. Modelling work determined that the EM sensor should have the ability to detect the difference between ferrite and pearlite even with such a small relative permeability ratio. Fig. 3(a) shows the microstructure from a Fe-0.8 wt% C sample after decarburising treatment of 1000°C for 2 hours, which consists of a surface ferrite zone, with a ferrite and pearlite mixed zone followed by fully pearlite on moving into the sample core. The sensor measured results in Fig. 3(b) show that inductance increases with increasing decarburising time (and hence decarburised depth) over the whole measured frequency range used (10 to 100 Hz). At a frequency of 10 Hz, the sensor could not readily distinguish the two samples with the least amount of decarburisation: decarburisation times of 10min (containing no separate ferrite layer but only a thin mixed zone), and 1 hour (containing a thin ferrite layer and a thicker mixed zone). By increasing the frequency these samples become distinguishable. Therefore, to detect thin decarburised layers, such as seen in industrial processing, the appropriate frequency needs to be chosen. This is understandable from the point of view that at very low frequency, if the skin depth is much larger than the thin decarburisation layer thickness, the contribution to the inductance from the decarburisation layer is too small compared to that from the core pearlite. On the other hand, if the skin depth is smaller than the decarburisation layer thickness, the variation of decarburisation layer thickness cannot be detected.
4. Conclusions Experiments and modelling show that decarburisation in steel rod samples can be measured using an EM sensor on-line during hot processing (by differences in permeability between surface ferrite and bulk austenite) or by off-line cold testing (by differences in permeability between surface ferrite and bulk pearlite). Appropriate testing frequency needs to be selected dependent on the decarburisation depth and whether on-line or off-line testing is being carried out to optimise signal output.
References [1] Papaelias MP, Strangwood M, Peyton AJ, Davis CL, Metall Mater Trans A 2004 (35A) 965-72 [2] Haldane RJ, Yin W, Strangwood M, Peyton AJ, Davis CL, Scripta Mater 54 (2006) 1761-65 [3] http://www.comsol.com/ [4] Thompson SM, Tanner BK, JMMM 132(1994) 71-78 [5] Thompson SM, Tanner BK, JMMM 123(1993) 283-298
90
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-90
Assessment of Grinding Damage on Gear Teeth using Magnetic Barkhausen Noise Measurements Moorthy VAIDHIANATHASAMY, Brian Andrew SHAW, Will BENNETT*, Peter HOPKINS* Design Unit, Newcastle University, Newcastle upon Tyne, UK *Ministry of Defence (Navy), Bristol, UK
Abstract. The marine Gears made with Case-carburised En36 steel were subjected to grinding damage during manufacturing. The MBN measurements have been made on different Gear teeth using three different methods, namely, High Frequency, Medium Frequency and Low frequency MBN measurements with the optimised measurement device and parameters so that the MBN signal from different depth ranges can be detected and analysed. The MBN measurements on these Gear teeth have shown that the grinding damage near the surface (< 10μm depth) can be detected using High frequency MBN, any sub-surface damage (within ~40μm depth) can be detected using Medium frequency MBN and the damage in the deeper layers (> 40μm depth) can be detected using Low frequency MBN measurements. The thermal damage caused by Grinding Burn is also clearly revealed by the shifting of the Low frequency MBN peak to lower magnetic field. Keywords. Magnetic Barkhausen Noise, Gears, Grinding damage.
1. Introduction The grinding damage induced during the final stage of manufacturing is a major concern affecting the quality and hence the fatigue life of Gears. It is known that the grinding damage is associated with alterations in Residual Stress (RS) distribution and the microstuctural state caused by thermal effects such as Burning or Rehardening. Conventionally, the grinding damage is assessed using Nital Etching method which reveals only microstructural changes on the surface. Often, the depth and the extent of the grinding damage may vary at different locations of the Gear teeth. In Casehardened steel Gears, it has often been found that the surface of the material may not reveal severe damage due to immediate cooling of the surface. But, the thermal damage and deformation may have altered the microstructure and RS in the sub-surface severely [1]. Since, the Magnetic Barkhausen Noise (MBN) signal is generated by the magnetization process which is strongly influenced by the microstructural and stress states of the ferromagnetic material, the MBN technique is considered as a potential NDT method to evaluate the grinding damage in ferromagnetic steels [2]. The MBN measurements can be made with different set of parameters, varying the maximum level and the excitation
M. Vaidhianathasamy et al. / Assessment of Grinding Damage on Gear Teeth
91
frequency of external magnetic field strength, the sensitivity of MBN pick-up coil, the analysing frequency range etc. All these factors decide the range of magnetisation and the depth from which the MBN signal is detected. In this study, three different MBN measurement methods have been compared for evaluating the depth range and extent of Grinding damage in carburised steel Gears. An attempt has been made to relate the three different MBN measurements with RS alteration below the surface at different depth ranges and also qualitatively assess the extent of thermal damage.
2. Experimental procedure The helical gears made from case-carburised En36 steel were subjected to different levels of damage during final grinding process. Small portions (25 mm long) of the teeth were cut from different locations of these Gears so that the Residual Stress (RS) – Depth profiles and the MBN measurements can be made using the existing X-ray diffraction system and the MBN devices at the Newcastle University. The three different MBN measurement methods, namely, High, Medium and Low frequency MBN measurements were made using three different set of measurement devices (electromagnetic yoke and MBN pick-up coil) and parameters (excitation frequency fex, maximum applied magnetic field Hmax and analysing frequency range, and signal amplification). The High frequency MBN measurements were made with MBN system and Gear probe supplied by Stresstech, Finland. The Medium and Low frequency MBN measurements were made with the MBN system and devices developed at Design Unit, Newcastle University, UK. The details of the High frequency MBN measurements (fex=125 Hz, Hmax= ±70 Gauss) and Low frequency MBN measurements (fex=0.2 Hz, Hmax=±300 Gauss) are given elsewhere [2-4]. The Medium frequency MBN measurements were made at 20 Hz magnetic excitation with maximum applied magnetic field strength of ±140 Gauss. The MBN signal was filtered using a 2 kHz high pass frequency filter and amplified to a Gain of 40 dB. The MBN signal profile is used for analysis. The skin depth, from which the MBN signals are detected, strongly depends on several measurement parameters such as the fex, Hmax, frequency response of the MBN pick-up coil, analysing frequency range of the MBN signals etc. in addition the effect of permeability and conductivity of the test materials. Due to the complex and synergistic influence of these factors, it is not possible to precisely determine the skin depth theoretically. However, it is well known that the skin depth of the MBN detection decreases with the increase in frequency of external magnetic excitation and the analyzing frequency range of MBN signals due to electromagnetic attenuation of the MBN signals within the test material. Previous studies [2-5] using the High and Low frequency MBN measurements made with differents set of parameters revealed that the high frequency MBN measurements did not detect changes in material properties beyond 10 μm depth whereas the low frequency MBN measurements detect changes in material properties to a depth of 600 μm. Based on the previous experiences, the High, Medium and Low frequency MBN measurements are expected to reveal the changes in material properties in the near-surface (<10 μm), subsurface (<40 μm) and deeper subsurface (upto ~ 400 μm).
92
M. Vaidhianathasamy et al. / Assessment of Grinding Damage on Gear Teeth
3. Results and Discussions It is expected that the comparison of High, Medium and Low frequency MBN measurements would indicate the possible distribution of residual stresses (RS) in the depth direction due to different skin-depth of the MBN signals generated in these measurements. In this paper, the comparison is shown with two examples. As an example 1, the MBN profiles measured using the three different types of measurements on a set of three different teeth from Gear S1 and their RS – Depth profiles are shown in Figure 1. The High frequency MBN profile shows no significant change in MBN peak among these three teeth indicating no significant variations in RS near the surface which is also supported by the RS-Depth profile. However, both the Medium and Low frequency MBN profiles show significant variations between them. The highest MBN peak for the Tooth-M indicates that it would have higher tensile RS in the subsurface region compared to other teeth. This is also evident from the RSDepth profiles shown in Figure 1(d).
M. Vaidhianathasamy et al. / Assessment of Grinding Damage on Gear Teeth
93
94
M. Vaidhianathasamy et al. / Assessment of Grinding Damage on Gear Teeth
300
Gear S1
-
(d)
Residual Stress, MPa
200 100 0 0
10
20
30
40
50
-100 Tooth N -200
Tooth M Tooth W
-300 Depth, Pm Figure 1. The MBN profiles measured with (a) High, (b) Medium and (c) Low frequency measurements and (d) RS-Depth profiles for three teeth from Gear S1. As an example 2, the comparison of High, Medium and Low frequency MBN profiles and the RS-Depth profiles for two teeth from Gears T1 and T3 are shown in Figure 2. In both the high and medium frequency MBN measurements, the T3-L tooth shows higher MBN level than T1-1 tooth. But, the low frequency MBN profiles show the opposite that the T1-1 tooth has higher MBN peak than T3-L tooth. The variations in high and medium frequency MBN profiles suggests that the T3-L tooth may have less compressive or more tensile RS than T1-1 tooth in the near-surface region (within 30μm depth). It can also be observed that the variation in high frequency MBN peak height shows a difference of ~ 40% and the variation in medium frequency MBN peak shows a difference of ~ 65% between for T1-1 and T3-L teeth. The larger difference shown by medium frequency MBN measurement indicates the presence of extended difference in RS profile even in subsurface layers (up to ~ 30 μm depth). It can be clearly seen from the RS-depth profiles that the T3-L tooth has more tensile RS than T1-1 tooth even at 20μm depth. But, at 40μm depth, the T1-1 tooth has tensile RS value while T3-L tooth has compressive RS value. The presence of more tensile RS in the deeper region is clearly reflected by the higher MBN peak value for T1-1 tooth than T3-L tooth in the low frequency MBN measurements. The distinct variations in the peak position of the Low frequency MBN profiles clearly show the extent of thermal damage resulting in microstructural softening among these Gear teeth. The higher applied magnetic field strength in the Low frequency MBN measurement maximizes the magnetisation range and hence reveals the extent of thermal damage by distinct shifting of the position of MBN profiles.
Average MBN level, % of 5V
M. Vaidhianathasamy et al. / Assessment of Grinding Damage on Gear Teeth
Carburised Gears T1 and T3 fex = 125 Hz 'fa = 70-200 kHz
30
(a)
20
25
95
Tooth-T3-L Tooth-T1-1
15 10 5 0 -100
-50
0
50
% of voltage applied to electromagnet
100
96
M. Vaidhianathasamy et al. / Assessment of Grinding Damage on Gear Teeth
200
Carburised Gears T1 and T3
(d)
Residual Stress, MPa
100 0 -100 0 -200 -300 -400
10
20
30
40
50
Tooth-T3-L Tooth-T1-1
-500 -600 -700 Depth, Pm
Figure 2. The MBN profiles measured with (a) High, (b) Medium and (c) Low frequency measurements and (d) RS-Depth profiles for teeth from Gears T1 and T3.
M. Vaidhianathasamy et al. / Assessment of Grinding Damage on Gear Teeth
97
4. Conclusions This study clearly shows that the difference in the RS distribution in the near-surface, subsurface and deeper regions can be identified by comparing the MBN profiles obtained from these three different MBN measurements. It is more appropriate to relate the MBN peak position to the extent of thermal damage and the peak height to the average RS variation over a certain depth depending on the type of MBN measurement and the parameters used. However, since the High and Medium frequency MBN measurements have limited effective magnetic field penetration resulting in smaller magnetisation range and they could not isolate thermal damage from the RS variations. References: [1] [2] [3] [4] [5]
B.A.Shaw, J.T.Evans and D.E.Yates, The influence of Grinding on the formation of Residual Stress Distribution in Ground Surfaces, Conference on Drives and Controls., Kamtech Publishing, UK, 1996, 21-26. V.Moorthy, B.A.Shaw, P.Mountford and P.Hopkins, Magnetic Barkhausen emission technique for evaluation of residual stress alteration by grinding in case-carburised En36 steel, Acta Materialia, 53 (2005) 4997-5006. V. Moorthy, B.A. Shaw and P. Hopkins, Surface and subsurface stress evaluation in case-carburised steel using high and low frequency magnetic Barkhausen emission measurements, J. Magnetism and Magnetic Materials, 299, 2006, 362-375. V. Moorthy, B.A. Shaw and P. Hopkins, Magnetic Barkhausen emission technique for detecting the overstressing during bending fatigue in case-carburised En36 steel, NDT&E international, 38, 2005, 159-166. V. Moorthy, B.A. Shaw, and K. Brimble, Evaluation of case depth in case-carburised gear steels using magnetic Barkhausen emission technique, Materials Evaluation, 62 (5) May 2004, 523-527.
98
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-98
Evaluation of Contact Fatigue Damage on Gears using the Magnetic Barkhausen Noise Technique Moorthy VAIDHIANATHASAMY, Brian Andrew SHAW, Will BENNETT*, Peter HOPKINS* Design Unit, Newcastle University, Newcastle upon Tyne, UK *Ministry of Defence (Navy), Bristol, UK Abstract. Gears made from Case-carburised SAE8620H steel were subjected to contact fatigue testing at different contact stress levels in the Gear Test Rig facility at Newcastle University. The High frequency Magnetic Barkhausen Noise (MBN) measurements were made at different intervals of fatigue cycles. The MBN signal level gradually increases with progressive fatigue cycles and the rate of change in MBN level systematically increases with the increase in contact stress level. However, at higher contact stress levels, the MBN level quickly reaches a maximum value and then starts to decrease with further fatigue cycles. This maximum MBN level may be considered as an indication of the critical stage of fatigue life beyond which a gear may be expected to fail soon. With increasing numbers of fatigue cycles, the large MBN activity occurs at lower magnetic field strength which clearly indicates the formation of soft magnetisation regions near the surface. This may be attributed to the deformation induced transformation of paramagnetic retained austenite into ferromagnetic martensite. Key words: Barkhausen Noise, Contact fatigue, Gears.
1. Introduction One of the most common modes of Gear failure is the contact fatigue damage which is commonly manifested as the initiation and progression of micro-pitting on the flanks of gear teeth. The progress of micro-pitting damage alters the Micro-geometry of Gear profile which in-turn alters the contact pattern of the Gear. This would introduce nonuniform high stress contact points and makes the Gear rotation more noisy, less efficient and prone to fatigue failure of the Gear teeth. The contact fatigue failure of the Gear normally occurs by the sudden breakage of the tooth by the crack propagation initiated from the Gear flank. Hence, the monitoring of contact fatigue using NDE method would be very useful in assessing the Gear condition and predicting the remaining life of the Gear.
M. Vaidhianathasamy et al. / Evaluation of Contact Fatigue Damage on Gears
99
The Magnetic Barkhuasen Noise (MBN) is the voltage pulses induced in the pick-up coil placed on the surface of the ferromagnetic material which is subjected to discrete changes in magnetization by the external varying cyclic magnetic field. It has been widely reported in the literature [1-3] that the MBN signal is very sensitive to changes in microstructural and stress states of the ferromagnetic steels. Since many medium and large size gears are manufactured using ferromagnetic steels, the MBN technique is considered as a potential NDT method for assessing the contact fatigue damage in Gears. This study has been carried out to understand and evaluate the variation in the MBN signal in response to progressive contact fatigue damage in case-carburised steel gears.
2. Experimental The contact fatigue tests have been carried out at Design Unit, Newcastle University, using 8 mm module, 20 teeth Varigears (Spur Gears with symmetrically varying toothwidth around the circumference – Figure 1) made with Case-carburised and Tempered SAE8620H steel [1], at 3000 rpm speed using OEP-80 Oil at 50qC as lubricant. Typical contact stresses for different tooth-width and torque levels are shown in Table 1.
Figure 1. Photograph of a VariGear
100
M. Vaidhianathasamy et al. / Evaluation of Contact Fatigue Damage on Gears
Table 1. Typical contact stresses for different tooth width and torque levels
Tooth Width, mm
Contact stress at 1300 Nm
Contact stress at 1900 Nm
MPa
MPa
28
1301
1517
25
1352
1581
23
1404
1645
21
1457
1711
19
1506
1773
18
1559
1848
The high frequency MBN measurements were made with commercially available MBN system and the Gear sensor containing ferrite-cored electromagnet and ferrite cored MBN pick-up coil supplied by Stresstech, Finland. The measurements were made at a magnetic excitation frequency of 125 Hz. Normally the MBN signals from a ferrite cored pick-up coil are generated in a wide frequency bandwidth ranging from excitation frequency to 1 MHz. Generally, avoiding the interference from higher harmonic contents of the excitation frequency and neglecting very small amplitude signals at high frequency end, the MBN signal is acquired in a appropriate frequency bandwidth. In this study, the MBN signal were acquired and analysed within the frequency range of 70-200 kHz considering the dominance of contact fatigue damage close to the surface. The total RMS voltage of the MBN signal multiplied by 200 represented as “MBN Display M value” and the average MBN signal profiles are used for analysis.
3. Results and Discussions The variations in MBN levels measured on six different teeth having different width and hence different contact stresses are shown in Figure 2 with progressive number of cycles at 1900 Nm and 1300 Nm Torque levels respectively. It can be observed that the MBN level increases rapidly in the initial stage and then slowly with progressive number of cycles. At higher stresses >1773 MPa, the MBN level reaches a maximum and then decreases in the later stages of fatigue life. With increase in number of fatigue cycles, the cyclic contact plastic deformation results in progressive micro-pitting of the gear surface as shown in Figure 3(a-c). The micro-pitting initiates micro-cracks on the surface against the sliding direction of the gear which grows into macro-crack below the surface along the rolling direction of the gear as shown in Figure 3(d). This results in macro-pit or failure of the gear teeth. This mechanism is influenced by other
M. Vaidhianathasamy et al. / Evaluation of Contact Fatigue Damage on Gears
101
complex gear running conditions such as changing contact stress distribution, lubrication condition, temperature, maximum bending stress, material quality and micro-geometry of the gear. This unpredictable failure event is evident from Figure 4 which shows only micro-pits on one tooth and a macro-pit above the pitch line on the adjacent tooth. This suggests that the catastrophic failure of the gear can occur without any prior warning.
MBN Display 'M' Value, A.U.
180 160 140
Tooth Width, mm Contact Stress, MPa
120
T1-28mm-1517 T2-25mm-1581
Gear- 4S Torque = 1900Nm MBN GAIN = 60
100 80
T3-23mm-1645 T4-21mm-1711 T5-19mm-1773
(a)
T6-18mm-1848
60 0
80
20 30 Number of million cycles
70 65
50
40
Gear- 5S Torque = 1300Nm MBN GAIN = 30 (b)
75 MBN Display 'M' Value, A.U
10
60
Tooth Width, mm Contact Stress, MPa
55
T11-28mm-1301
50
T12-25mm-1352
45
T13-23mm-1404
40
T14-21mm-1457 T15-19mm-1506
35
T16-18mm-1559
30 0
10
20
30 40 Number of million cycles
50
60
70
Figure 2. The variations in MBN level with progressive number of cycles at (a) 1900 Nm and (b) 1300 Nm on six different teeth having different widths and contact stresses. Note the MBN signal amplification gain for (a) is 60 while it is 30 for (b).
102
M. Vaidhianathasamy et al. / Evaluation of Contact Fatigue Damage on Gears
Figure 3. The photographs of the flank of 18 mm width tooth of the gear- 4S showing the progressive micro-pitting (Grey strain area) after (a) 8m, (b) 20m and (c) 34m cycles at 1900 Nm and (d) micro-graph showing typical crack growth below the gear flank surface.
Figure 4. The photograph of gear showing only micro-pitting on one tooth and a large macro-pit failure on the adjacent tooth.
M. Vaidhianathasamy et al. / Evaluation of Contact Fatigue Damage on Gears
103
Normally, a gear is considered as failed either when there is loss of 20μm thickness of gear flank profile caused by micro-pitting or when there is greater than 4% area of macro-pits on the gear. However progressive contact fatigue damage has not been directly related to changes in metallurgical properties such as hardness or microstructure, even though, they may be affected and causes changes in MBN level. Hence, this study attempts to monitor the changes in MBN level with progressive contact fatigue. The variations in the MBN level with progressive number of cycles at lower contact stresses (in the range of 1301 to 1559 MPa) clearly suggest that the initial increase in MBN level is also very gradual and systematic in response to stress level with progressive number of cycles. This suggests that the contact fatigue damage can be detected in this type of gear steels at very early stage using the MBN technique well before the development of any visible surface damage. Since the nature of gear failure is highly unpredictable and catastrophic in many cases, the transition of MBN level from a maximum may be considered as an indication of the critical stage beyond which the failure can occur at any time depending on other unknown parameters. The high frequency MBN profiles measured at the dedendum of 28 mm and 18 mm width teeth at different number of cycles are shown in Figure 5. It can be observed that the high frequency MBN level increases with number of cycles in 28 mm width tooth whereas in 18 mm width tooth, the MBN level reaches a maximum after 8 m cycles and then decreases with progressive number of cycles. Also, in both cases, initially the MBN peak position shifts to lower applied voltage (magnetic field) and then again shift back to slight higher field. The increase in MBN with shifting of peak to lower field could be due to the combined effects of deformation induced transformation of retained austenite into martensite and fatigue softening. The carburised gear surface contains about 25% volume fraction of retained austenite phases which is a paramagnetic meta-stable phase. During running, the gear surface is subjected to micro-plastic deformation which transforms the metastable retained austenite into martensite. Since, the transformed martensite is a ferromagnetic phase, it results in nucleation and movement of additional magnetic domain walls which effectively contribute to increase in MBN level. The initially hard tempered martensite poses high density of tangled dislocations. The cyclic deformation could cause this tangled dislocation to rearrange into dislocation cells. The domain walls can move with relatively less restraint within the dislocation cells compared to tangled dislocation structure. This could contribute to increased MBN level with peak shifting to lower field. The reduction in MBN from maximum level and the shifting of peak position back to slightly higher field could be due to the effects of cyclic plastic deformation induced formation of more compressive residual stresses and cyclic hardening of the microstructure. After certain number of cycles at a given stress level, the transformation of retained austenite to martensite would be completed. Normally, the number of fatigue cycles required for complete transformation of meta-stable retained austenite increases with decrease in contact stress level. This also depends on other factors like temperature, lubrication condition etc. Once the phase transformation is complete, the continued cyclic plastic deformation of near-surface could generate additional dislocations which could accumulate around the dislocation cell walls and that results in the reduction of size of dislocation cell interior. This could cause decrease in the displacement length of magnetic domain walls and stronger pinning of
104
M. Vaidhianathasamy et al. / Evaluation of Contact Fatigue Damage on Gears
domain walls at the dislocation cell walls. This could contribute to the decrease in the MBN level from maximum and shifting of the MBN peak back to higher field. The effect of contact stress level on the rate of changes in the material behaviour introduced by these deformation processes is clearly reflected in the MBN profiles (Figure 5). At lower stresses, the effect of transformation of retained austenite into martensite would dominate and cause gradual increase in the MBN level. However, at higher contact stresses, the phase transformation would complete after smaller number of cycles. With progressive number of cycles, the cyclic-plastic deformation and the residual stress alteration would have dominant effect. Hence, the MBN level would increase to a maximum after certain number of cycles and then would decrease with progressive number of cycles as observed in Figure 5.
Figure 5. The high frequency MBN profiles measured at the dedendum of (a) 28 mm and (b) 18 mm width teeth at different number of cycles.
M. Vaidhianathasamy et al. / Evaluation of Contact Fatigue Damage on Gears
105
Even though this explanation seems to be appropriate, very large (> 100%) increase in MBN level compared to smaller volume fraction (~25%) of retained austenite indicates that some predominant form of magnetic softening taking place in this steel by complex dislocation substructure evolution with progressive contact fatigue deformation. It requires other metallurgical investigations to answer this anomalous and surprise MBN behaviour.
4. Conclusions This study shows that the MBN technique can be used to detect the changes in the Gear caused by contact fatigue damage even at very early stages of fatigue life. The effect of variation in the contact stress level is also clearly reflected by gradual and systematic changes in the MBN level and its rate of change with progressive number of fatigue cycles. The overall response of the MBN suggests that the MBN level increases to reach a maximum level and then slowly decreases with progressive number of fatigue cycles. This is attributed to the initial deformation induced transformation of retained austenite to martensite and fatigue softening followed by cyclic plastic deformation induced hardening. References [1] [2] [3]
T.R. Hyde, J.T. Evans, B.A. Shaw, Effect of stress and heat treatment on magnetic Barkhausen emission in case-carburised steels, Mater. Eval., 58(8)(2000) 985-990. L.P.Karjalainen, M.Moilanen, Fatigue softening and hardening in mild steel detected from Barkhausen Noise, IEEE Trans. Magn., MAG-16 (3) (1980) 514-517. V.Moorthy, B.K.Choudhary, S.Vaidyanathan, T.Jayakumar, K.Bhanu Sankara Rao, Baldev Raj, An assessment of low cycle fatigue damage using magnetic Barkhausen emission in 9Cr-1Mo ferritic steel., Int J. Fatigue, 21 (1999) 263-269.
This page intentionally left blank
Inverse Problems
This page intentionally left blank
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-109
109
3D Reconstruction of flaws in metallic materials by eddy currents inspections Alessandro PIRANIa, Marco RICCIa, Antonello TAMBURRINOb, Salvatore VENTREb,1 a Polo Scientifico Didattico di Terni, Università degli Studi di Perugia, Via Pentima Bassa 21, Terni 05100, Italy b Ass. EURATOM/ENEA/CREATE,DAEIMI, Università degli Studi di Cassino, Via G. Di Biasio 43, Cassino 03043, Italy
Abstract. This work is focused on the image reconstruction of defects in metallic materials using time-harmonic eddy currents testing measurements. The proposed approach combines an efficient numerical model of the probe-defect interaction and a least square error regularized procedure for solving the inverse problem. The method has been successfully tested to detect multiple volumetric defects on multiple layers of a planar conductive material. The regularization term is the total variation, selected to “encode” the a priori information that defects are supposed to be “blocky”. In this manner, the method is potentially capable of treating on the same foot several defects type such as EDM, fatigue crack, stress corrosion crack etc. Keywords. Eddy currents, nondestructive evaluation, total variation regularization, numerical simulation.
1. Introduction Eddy currents non-destructive techniques are widely used in the field of electromagnetic inspection of metallic structures to determine their composition and to detect possible flaws. In this framework, a main issue is the ability to assess the 3D conductivity profile of the sample under test. The major difficulty encountered to achieve this aim is the non-linearity and ill-posedness of eddy currents inverse scattering models. In the present work, we tackle this issue by combining an efficient numerical model of the probe-defect interaction and a total variation procedure for solving the inverse problem and reconstructing the 3D conductivity profile of flawed samples. Our approach exploits a multi-position and a multi-frequency measurement system and it has been tested on synthetic noisy data as preliminary proof in the perspective of an experimental application to real defects. Here we assume that the defects are volumetric with a finite resistivity. The modeling of volumetric defects, as opposed to the modeling of zero-thickness defects, is more intriguing and is receiving increasing attention [1]–[7]. Here we present an efficient integral numerical model where the unknown is 'J, the eddy current variation due to the presence of defects. The methods is in the same line of the approaches 1 Corresponding Author: Salvatore Ventre, Università degli Studi di Cassino, Via G. Di Biasio 43, Cassino 03043, Italy; E-mail:
[email protected]
110
A. Pirani et al. / 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections
presented in [1] and [8] where perfectly insulating volumetric and zero-thickness defects are treated. The numerical calculation of 'J combines several advantages, among them: (i) requires a local discretization in a neighborhood of the defect only, (ii) the integral formulation involves the static free-space Green function. The inverse problem in cast in term of minimization of the discrepancy, that is the least square error between the experimental and numerical computed data. Due to the intrinsic ill-posedness of the problem, we include a proper penalty term “encoding” a priori information about the defects. Our choice is fall on the Total Variation (TV) regularization term that penalizes functions with great spatial variability with respect to “blocky” functions, while preserving the edges [9-11]. The TV has been chosen because it accounts for the a priori information that the anomalies are blocky. The paper is structured as follows: the finite element method used to solve the forward electromagnetic problem is presented in Section 2, the inversion algorithm is presented in Section 3 and numerical results are presented in Section 4.
2. Forward Problem The numerical method here proposed has been developed in order to treat efficiently the typical situation encountered in eddy current testing where anomalies are present in an a priori known sub-region VT of a conducting domain VC. The anomalies perturb locally the induced eddy current J and, therefore, it is very efficient [1, 8] to assume as unknown 'J=J-J0 where J0 is the eddy current when the material is flawless. Specifically, by combining the electric field expressed in terms of the vector and scalar potentials with the constitutive relationship we obtain:
KJ K0J 0
jZA>J @ M jZA ext , in VC
(1)
jZA 0 >J 0 @ M 0 jZA ext , in VC
where J, J 0 L2div VC , J A : vr o
P0 4S
J0
0 in VC J nˆ
vr '
³ r r' dV ,
0, J 0 nˆ
0 on wVC ,
(2)
VC
K is the electrical resistivity of the conductor (in the presence of the defect), Aext is the vector potential produced by the inducing coil, M is the scalar potential, the subscript 0 refers to the configuration in the absence of defects (defects are modeled as a perturbation 'K of the electrical resistivity, i.e. K=K0+'K). From (1) it follows the equation for 'J: K'J jZA>'J @ 'KJ 0 'M , in VC
(3)
where 'M=M-M0. The related numerical model is based on [12]. Specifically, the unknown is represented as 'J ¦kAE 'I k u Tk where Tk is an edge-element shape function, and AE is a
A. Pirani et al. / 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections
111
proper subset of the edges of the graph made by nodes and edges of the finite element mesh. Choosing properly this subset it is possible to impose the gauge and boundary condition. Moreover, since 'J is localized in a neighborhood of the defect, it is possible to use a local discretization of the conductive material thus achieving a great reduction in the computational cost [1, 8]. The numerical model is, finally, obtained by imposing (3) in weak form:
³
VCLOC
u N k (K'J jZ A>'J @)dV
³
VCLOC
u N k 'KJ 0dV
N k .
(4)
In (4) VCLOC is a local region in a neighborhood of the tentative region VT
V
VCLOC VC where 'J is not vanishing, and we exploited that the term involving 'M gives no contribution thanks to the solenoidality of the test functions and their vanishing normal component on the boundary. The corresponding linear system is: T
Z 0 'R 'I
'RI 0
(5)
where, Z0=R0+jZL, 'I is the column vector of the coefficients representing the expansion of 'J and L ij
'R ij
P0 4S
u N i ( x) u N j ( x' )
³ ³
x x'
VCLOC VCLOC
³uN
i
³uN
i
(7)
K 0 u N j dV
(8)
J 0 dV
(9)
VCLOC
I 0,k
³uN
k
(6)
'K u N j dV
VCLOC
R 0,ij
dV dV '
VCLOC
Once the induced current density perturbation 'J has been computed, it is possible to compute the related voltage induced on the coil. Finally, it is worth noting that the unperturbed current density J0 can be computed analytically for canonical geometries or numerically for more complicated configurations.
3. Inverse Problem We assume that the measurement consists of the value of time-harmonic measurements of the (complex) voltages induced on the exciting coil due to the presence of the anomalies. Specifically, the data is the column array V * consisting of measurements collected at different locations and frequencies (we simultaneously process all of them to retrieve the overall 3D conductivity profile).
112
A. Pirani et al. / 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections
The proposed inversion method cast the problem in terms of minimization. Specifically, the solution of the inverse problem is the minimizer of E x
2
V * V x DTV x
(10)
where x is the column vector containing the parameters describing the conductivity V=K-1 (here assumed uniform in each element of the finite element mesh) V * and V x are the measured and numerically computed voltages variation due to the presence of anomalies, D is the regularization parameter and TV is the total variation regularization term [9-11] defined as TV x
³
VT
V dV
(11)
where V is the conductivity represented by x. The total variation penalty term, introduced as regularization term, penalizes function with great spatial variability but preserving the edges [9-11] and, therefore, it is indicated when the unknown is “blocky” as in the present problem. The implemented inversion algorithm update iteratively the current solution x(n) at step n with the following rule: x n 1
x n 'x n
(12)
where 'x n minimizes E n 1 'x
2
V * V x n S n 'x DTV x n 'x
(13)
S n being the sensitivity map arising from the linearization of V x in a neighborhood
of x(n). The elements of the “sensitivity” matrix S n represent the derivatives of the probe voltage with respect to the voxels’ conductivity. In the present work we compute the sensitivity by using the method described in [13], that results in a first-order Born approximation of the electric field inside voxels [14]. A closed expression for 'x n that minimize E n 1 is not available, thus for each iteration n of the overall inversion algorithm, a further iterative minimization procedure, labeled henceforth by the index Q must be carried out. In the present work we employ the Lagged Diffusivity Fixed Point Iteration Method introduced by Vogel and Oman [10, 11]. The choice of a suitable value for the regularization parameterD is of utmost importance. We applied the L-curve method for choosing the regularization parameter (see figure 1(left)). Specifically, defining Deq as the value that balances the LSE and the TV regularization term, we found that the point of highest curvature, giving the value of the regularization parameter, is close to 10-3 uDeq.
A. Pirani et al. / 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections
113
Figure 1. Left: L-curve analogous for the TV regularization. Right: Typical graph of the TV error vs. the TV parameters. Both graphs refer to defect type I.
We have also analyzed the behaviour of E n 1 when D and Q are varied, setting 'x to the value that minimizes the overall error in the spanned range of parameters D and Q. Figure 1 (right) show the typical error trend where the solid curve identifies the value D* that minimizes E n 1 . We found that D* is resulted to be very close to the value provided of the regularization parameter provided by the L-curve method. Figure 1 refers to defect type I (see figure 3). Similar results have been attained for a wide variety of numerical cases with different defect types and noise levels. Since the data are provided by a multi-frequency measurement system, we have properly weighted each frequency in order to gain useful information from all of them. To accomplish this aim, we operated a frequency dependent normalization of V and S. Usually the weights are related to the energy of the signal at the corresponding frequency, on the contrary we carry out a normalization based on a SVD analysis of the sensitivity matrix at single frequencies. This normalization is modified to take into account the presence of additive synthetic noise: in this case the weights are determined both from the SVD analysis and from the data noise variance. Finally, to avoid instabilities in the reconstruction, as well as to enhance the convergence speed, we introduce a priori information about the conductivity range of values. Specifically, when in a given element the conductivity (represented by x(n)) is greater than the value of the host material, we set it to the value of the host material. A similar processing is carried out when the conductivity assumes negative values.
4. Numerical Results In this section we consider an Aluminium plate (thickness 3mm, V=37.7u106S/m) and we focus on the conductivity retrieval in a small region (VT) of 12mmu12mmu3mm, modelled with a 3D regular grid of cubic voxels having the edge of 1mm. Defects are approximated by a well defined number of voxels with fixed conductivity. The probe consists of a coil with the following characteristics: inner radius 0.5mm, outer radius 2mm, height 3mm, 200 turns, lift-off 0.5mm. In the procedure the probe is placed in 25 different positions, whose centres build up a regular grid of points oriented at 45 degrees respect to the x axis and equally spaced at a distance of about 2mm that
114
A. Pirani et al. / 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections
corresponds to the coil outer radius, guaranteeing data independence and optimal covering of the voxel region. The multi-frequency excitation is contextually exploited in order to inspect the specimen with varying resolution and to examine its inner structure at different depths. Since any frequency is associated to a specific skin depth penetration G, we adopt three different values (670, 1500, 6000 Hz) whose skin-depths correspond to the layer depths. In eddy-currents applications the coil voltage variation due to a defect may be a very small part (0.01%- 0.0001%) of the absolute coil voltage. Since the eddy currents intensity is proportional to the excitation frequency, as the inspection depth increases, i.e. the operation frequency decreases, the relative voltage variation decreases and the SNR tends to be determined mainly by the unavoidable limitations of the measuring apparatuses, usually determined from its operating range. In order to be consistent with these considerations, we have introduced a synthetic noise, in the numerically computed voltages vector, represented by an uncertainness circle in the voltage complex plane which radius is proportional to the coil voltage in air, Vair. Henceforth * * V * VNF n , where VNF (n) is the noise free data array (noise array) and noise level stands for the ratio between the uncertainness circle radius and the magnitude of Vair. To gain insight about the actual noise magnitude compared to the defect signal contribution, Table 1 reports some indicative values concerning defect types I and II for the noise level adopted (noise level = 0.0005 % ). Specifically, for a given frequency, * * signal level is the ratio between the L1-norm of the voltage variation GV * VNF VBG due to the defect and the coil voltage in air, whereas relative noise is the ratio between * the L2-norm of the noise n and GV * . Here VBG is the so-called background voltage, that is the coil voltage when defects are not present. Figure 2(left) shows the trends of the total normalized error LSE versus the overall iteration index n, having rescaled to one the value at n=1. As expected, the LSE tends to decrease as the iterations go on. Usually, in order to stop the overall inverse procedure, a proper LSE error threshold, related to the value of the actual precision of the experimental measurement, is prescribed. For noisy data, the error asymptotic value mainly depends on the chosen noise level, and then the threshold has been selected once a time. In figure 2(right) we report a plot of D* vs. Deq for different defect types and noise levels: we note that D* always belongs to a neighbourhood of 10-3uDeq. Moreover, as the noise level increases, the parameter Deq tends to assume a constant value for all tests. Figure 3 shows some reconstructed conductivity maps with and without additive noise. The contribution of a deep defect to the total error is weaker than the one of a superficial defect and, at a fixed depth of inspection, high-conductivity defect is harder to reconstruct than a low-conductivity one. Nevertheless the results show that the conductivity profiles are satisfactory assessed in few iterations. Table 1. Signal level and Relative Noise
Signal level Freq.[Hz] 670 1500 6000
Defect Type I 0.00573 % 0.0192 % 0.0995 %
Defect Type II 0.00279 % 0.00830 % 0.0154 %
Relative noise Defect Type I 12.8 % 3.2 % 0.8 %
Defect Type II 25.4 % 7.1 % 4.5 %
A. Pirani et al. / 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections
115
Figure 2. Left: typical trends of the error LSE vs. the iterations, for no-noise and noisy data: the square signs and the circle ones refer to the defect type I and type II respectively (see also Figure 3). The noisy data are obtained with a noise level equal to 5u10-6. Right: plot of D vs. Deq for different defect types and noise levels. The marks refer to no-noise tests (squares), noise levels 10-6 (triangles), 5u10-6 (stars) and 10-5 (circles).
Figure 3. Examples of reconstructed conductivity map for two defect types: 1st column reports the actual maps; 2nd and 3rd columns report the maps obtained by processing no-noisy data for a threshold fixed at 10-4 and 10-6 respectively; in the 4th column we show the maps obtained at the stop iteration (6th and 4th) by processing noisy data with a noise level of 0.0005 %. The stopping iterations refers to a threshold fixed at 5u10-4 and 5u10-3 respectively.
116
A. Pirani et al. / 3D Reconstruction of Flaws in Metallic Materials by Eddy Currents Inspections
5. Conclusions In this work we have addressed the imaging of 3D volumetric defects by eddy current testing. Specifically, we have proposed an efficient integral numerical formulation where the unknown is 'J, the eddy current variation due to the presence of defects. The method combine several advantages: (i) it requires a local discretization in a neighborhood of the defect only and (ii) the integral formulation involves the static free-space Green function. The inverse problem, on the other hand, has been cast in term of minimization of the LSE plus a Total Variation regularization term. The Total Variation term accounts for the a priori information that the defect are piecewise constant.
Acknowledgements This work was supported in part by the Italian Ministry of University (MIUR) under a Program for the Development of Research of National Interest (PRIN grant # 2004095237) and in part by the CREATE consortium, Italy.
References [1]
[2] [3] [4] [5] [6] [7] [8] [9] [10] [11] [12]
[13]
[14] [15]
M. Morozov, G.Rubinacci, A.Tamburrino, S.Ventre, “Numerical Models of Volumetric Insulating Cracks in Eddy-Current Testing With Experimental Validation”, IEEE Trans. Mag., Vol. 42, No. 5, May 2006, pp. 1568-1576. J. R. Bowler, S. A. Jenkins, L. D. Sabbagh, and H. A. Sabbagh, “Eddy current probe impedance due to a volumetric flaw,” J. Appl. Phys., vol. 70, no. 3, pp. 1107–1114, 1991. Z. Badics, J. Pavo, H. Komatsu, Y. Matsumoto, and K. Aoki, “Fast flaw reconstruction from 3d eddy current data,” IEEE Trans. Magn., vol. 34, no. 5, pp. 2823–2828, Sep. 1998. Z. Badics, J. Pavo, Y. Matsumoto, and H. Komatsu, “Forward solution speed-up for 3D eddy current inversion,” IEEE Trans. Magn., vol. 36, no. 4, pp. 1124–1127, Jul. 2000. D. Reis, M. Lambert, and D. Lesselier, “Eddy-current evaluation of three-dimensional defects in a metal plate,” Inverse Problems, vol. 18, pp. 1857–1871, 2002. D. Prémel and A. Baussard, “Eddy-current evaluation of three-dimensional flaws in flat conductive materials using a Bayesian approach,” Inverse Problems, vol. 18, pp. 1873–1889, 2002. Y. Li, L. Udpa, and S. Udpa, “Three-dimensional defect reconstruction from eddy-current NDE signals using a genetic local search algorithm,” IEEE Trans. Magn., vol. 40, no. 2, pp. 410–417, Mar. 2004. R. Albanese, G. Rubinacci, F. Villone, “An integral computational model for crack simulation and detection via eddy currents”, J. of Comp. Phys., Vol. 152, pp. 736-755 (1999). L. I. Rudin, S. Osher , and E. Fatemi, Nonlinear total variation noise removal algorithms, Proc. of the 11th Annual International Conference the center for Nonlinear Studies, 60, (1992) 259-268. C. R. Vogel and M. E. Oman, Iterative methods for total variation denoising, SIAM J. Sci. Comput. 17 (1), (1996) 227–238. C. R. Vogel, Computational Methods for Inverse Problems, SIAM: Frontiers in Applied Mathematics 23, (2002) R. Albanese and G. Rubinacci, “Finite element methods for the solution of 3D eddy current problems” in Advances in Imaging and Electron Physics, Peter W. Hawkes (ed.), vol. 102, (Academic Press), 1998, pp. 1-86. D. N. Dyck, D. A. Lowther, and E. M. Freeman, A Method of Computing the Sensitivity of Electromagnetic Quantities to Changes in Materials and Sources, IEEE Trans. On Magnetics, 30, 5 (1994). S. M. Nair and J. H. Rose, Reconstruction of three-dimensional conductivity variations from eddy current (electromagnetic induction) data, Inverse Problems, 6, (1990) 1007-1030. R. Fletcher and C. M. Reeves, Function minimization by conjugate gradients, The Computer Journal, 7 (2), (1964) 149-154.
Electromagnetic Nondestructive Evaluation (XI) A. Tamburrino et al. (Eds.) IOS Press, 2008 © 2008 The authors and IOS Press. All rights reserved. doi:10.3233/978-1-58603-896-0-117
117
Multi-frequency Eddy Current Imaging for the Detection of Buried Cracks in Aeronautical Structures Yohan LE DIRAISON and Pierre-Yves JOUBERT SATIE, ENS Cachan, CNRS, UniverSud 61 av. du President Wilson, 94235 CACHAN Cedex, FRANCE Abstract. The authors present a signal processing method dedicated to the detection of defects buried next to rivets in aeronautical lap joints