WOOD AND CELLULOSIC CHEMISTRY second edition, revised and expanded
edited by
David N.-S. Hon Clemson University Clems...
169 downloads
2275 Views
97MB Size
Report
This content was uploaded by our users and we assume good faith they have the permission to share this book. If you own the copyright to this book and it is wrongfully on our website, we offer a simple DMCA procedure to remove your content from our site. Start by pressing the button below!
Report copyright / DMCA form
WOOD AND CELLULOSIC CHEMISTRY second edition, revised and expanded
edited by
David N.-S. Hon Clemson University Clemson, South Carolina
Nobuo Shiraishi Kyoto University Kyoto, Japan
M A R C E L
MARCEL DEKKER, INC. U E K K E R
NEWYORK BASEL
Library of Congress Cataloging-in-Publication Data
Woodandcellulosicchemistry / editedbyDavidN.-S.Hon, Nobuo Shiraishi.-2nded.,rev.and expanded. p. cm. Includes index. ISBN 0-8247-0024-4 (alk. paper) 1. Cellulose. 2.Wood-Chemistry. I. Hon,David N.-S. 11. Shiraishi,Nobuo. QD323.W662000 572'.56682"dc21 00-060
This book is printed
o n acid-free paper.
Headquarters
Marcel Dekker, Inc. 270 Madison Avenue, New York, NY 1 0016 tel: 2 12-696-9000; fax: 2 12-685-4540 Eastern Hemisphere Distribution
Marcel Dekker AG Hutgasse 4, Postfach 812, CH-4001 Basel, Switzerland tel: 41-61-261-8482; fax: 41-61-261-8896 World Wide Web
http://www.dckker.com The publisher offers discounts on this book when ordered in bulk quantities. For n1ore infornmation. write to Special Sales/Professional Marketing at the headquarters address above. Copyright 0 2001 by MarcelDekker,Inc.
All RightsReserved.
Neithcr this hook nor any part nuy be reproduced o r transmitted in any form or by any means. electronic o r mechanical, including photocopying. microlilnling. and recording. o r by any information storage and retrieval systcm. without permission in writing from the publisher. Current printing (last digit): 1 0 9 8 7 6 5 4 3 2 1 PRINTED IN THE UNITED STATES OF AMERICA
Preface
Life and its surroundings are constantly changing within our dynamic world. As we stride into the new millennium, information technology and biotechnology continue to flourish. Rapid economic expansion, social development, and high demands for shelter, clothing, energy, and food for our overpopulated world have resulted in a desperate need for new and yet functional materials to support society’s infrastructure. Wood or lignocellulosic-based materials have made a significant contribution to the quality of living for human beings. With new developments in wood chemistry, scientists are confident that wood will continue to play an important role in fulfilling the needs of human beings. Over the past decade, the trend of emphasizingbio-basedtechnologieshasbeen observed worldwide. In February 1998, a long-term development project, PlanVCrop-based Renewable Resources 2020, was implemented among the U.S. Department of Agriculture, U.S. Department of Energy, and many U.S. companies, agricultural associations, and universities. The aim of the project was to obtain novel chemicals from plant- and crop-based renewable resources in order to widen the usage of crops, the yield of which has been significantly increased through bio-technological advancements. The recent movement of producing foods by means of genetically manipulated seeds should enhance the effectiveness of this project. Before the start of this project-which is considered the future of the petrochemicalindustry-majorchemicalcompanies in the UnitedStates,suchasDow Chemical,Dupont, and Monsanto,havebeenchanging their strategies in research and development.Theyhavestrengthened their bio-basedresearch field, trying to yield as many chemicals as possible from biomass. They are developing production technologies for ethanol, sorbitol, lysine, tryptophane, citric acid, lactic acid, poly(lactic acid), erythritol, 1,3-propanediol,etc.,frombiomass.Furthermore, in August of 1998 PresidentClinton issued an executive order, “Developing and Promoting Biobased Products and Bioenergy,” to further the development of a comprehensive national strategy that includes research. development, and private sector incentives to stimulate the creation and early adoption of technology needed to make bio-based products and bio-energy cost-competitive in national and international markets. Also. there has been research in so-called “green chemistry.” In this new methodology. biomass is the recommended MW material. Thc importance of wood and cellulose rescarch is thus rccognizcd. iii
iv
Preface
Since the publication of' the first edition of this book, considerablc advancement i n various fields ofwood chemistry has been made, as can be attested by many scientific publications in addition to well-attended international conferences. We contacted the contributors to the first edition, soliciting their opinions on revising and updating the book, and we received tremendous support from them as well as the publisher. Unfortunately, and inevitably, several authorswereunableto participate, buttheyrccomrnended their successors. Although most of the chapters in this new edition carry the same titles as those i n the previous edition, they have all been extensively revised and updated. In addition, this edition includes several new chapters representing important threads in the total fabric of wood chemistry. These new chapters cover the subjects of chemical synthesis of cellulose, preservation of wood, preservation of waterlogged wood, biodegradable polymers from lignocellulosics, recycling of wood and fiber products, and pulping chemistry. As editors, we feel fortunate to have been able to recruit some of the best talent in the field to this endeavor. We thank the contributors for their efforts. Any praise for the content should be addressed to them, and comments and criticisms to us will be welcome.
David N.-S. Hon NoDuo Shiruishi
Contents
1.
Ultrastructure and Formation of Wood Cell Wall
1
Minoru Fujittr trrlcl Hirnshi Hcrmdrr
2.
ChemicalComposition and Distribution
SI
Shirr) Strkrr
3.
Structure o f Cellulose: Recent Developments in Its Characterization
83
Frrrtlittrktr Hot-ii
4.
Chemistry of Lignin 109 Akirn Srrkrrkihrrr-rrcrrlrl Yoshillit-o Strrlo
S. Chemistry of Cell Wall Polysaccharides
175
Ttrtltrslli lsllii rrrltl Kuxrt1tr.w Shirr1i:rr
6.
Chemistry of Extractives Toshitrki U r ~ r t w ~ ~ r
7.
Chemistry of Bark
2 13
243
Kokki Sakoi
8. ChemicalCharacterization o f Wood and Its Components
275
Jrrirtw Htrexr cult1Jucrrlittr Frret-
9.
Color
IO.
3x5 NoDrryrr Mitlcwlrr.cr
~ t n dDiscoloration
D m i t l N . -S. Horl
trrld
Chemical Degradation
443
Krcrrl-ZotrgLrri
1 I. Weathering and Photochemistry o f Wood IltrlGcl N.-S. Hot1
S I3
V
vi
Contents
12. Microbial, Enzymatic, and Biomimetic Degradation of Lignin in Relation to Bioremediation 547 Rrkqfumi Huttnri und Mikio Shimadu 13. Chemical Modification of Wood
573
Misato Nothoto
14. Chemical Modification of Cellulose599 Akirn Isogai
15.
ChemicalSynthesis of Cellulose627 Furniaki Nukatsubo
16. Wood Plasticization
655
Nohuo Shiruishi
17. Wood-Polymer Composites
701
Hirnshi Mizunztrchi
18.
Adhesion and Adhesives
733
Hiroslli Mizurturc.hi
19. Pressure-SensitiveAdhesives and Forest Products765 Hiroshi Mizunlcrchi
20. 21.
Wood-InorganicCompositesas Shiro Suku Preservation of Wood
Prepared by the Sol-Gel Process
795
D u r r d D . NicAolcrs
22.
Preservation of Waterlogged Wood
807
David N.-S. Hot1
23.
Biodegradable Plastics from Lignocellulosics Muriko Yr)shioku m c l Nohuo Shirtrishi
74.
Recycling o f Wood and Fiber Products849 Tcrkcrrlori Arirrrn
25.
Pulping Chemistry 859 Giirn11 Gelle~rstcclt
827
781
Contributors
TakanoriArima Department of Biomaterial Sciences, Graduate School and Life Sciences, The University of Tokyo, Tokyo, Japan
of Agricultural
Jaime Baeza Departamento de Quimica, Facultad de Ciencias, Universidad de Concepcicin, Concepcicin, Chile Juanita Freer Departamento de Quimica, Facultad de Ciencias, Universidad deConcepcicin, Concepcicin, Chile Minoru Fujita Division of Forest and BiomaterialsScience,Graduate culture, Kyoto University, Kyoto, Japan Goran Gellerstedt Department of Pulp and PaperChemistry Institute of Technology, Stockholm, Sweden
School of Agri-
and Technology, Royal
Hiroshi Harada Division of Forest and Biomaterials Science, Graduate School riculture, Kyoto University, Kyoto, Japan
of Ag-
TakefumiHattori
Wood Research Institute,Kyoto University, Kyoto, Japan
David N.-S. Hon Carolina
School of Nature Resources, Clernson University, Clemson,South
FumitakaHorii
Institute for Chemical Research,
Kyoto University, Kyoto, Japan
TadashiIshii Division of Bio-Resources Technology, Forestry and Forest Products Research Institute, Ibaraki, Japan Akira Isogai Department of Biomaterial Science, The University of Tokyo, Tokyo, Japan Yuan-Zong Lai Faculty of Paper Science and Engineering, SUNY College of Environmental Science and Forestry, Syracuse, New York vii
viii
Contributors
NobuyaMinemura
Hokkaido Forest Products Research Institute,Hokkaido, Japan
Hiroshi Mizumachi
Professor Emeritus, The University of Tokyo. Tokyo, Japan
FumiakiNakatsubo Division of Forest and BionlaterialsScience,GraduateSchool Agriculture, Kyoto University. Kyoto, Japan Darrel D. Nicholas State, Mississippi MisatoNorimoto
Forest Products Laboratory, Mississippi State University, Mississippi
Wood Research Institute, Kyoto University, Kyoto. Japan
Shiro Saka Department of Socio-Environmental Energy Science,GraduateSchool Energy Science, Kyoto University, Kyoto, Japan KokkiSakai
of
of
Faculty of Agriculture, Kyushu University. Fukuoka, Japan
AkiraSakakibara Laboratory o f Wood Chemistry. Research Group of Bioorganic Chemistry, Division of Applied Bioscience, Hokkaido University. Sapporo. Japan Yoshihiro Sano Laboratory of Wood Chemistry. Research Group of Bioorganic Chemistry, Division of Applied Bioscience, Hokkaido University, Sapporo, Japan Mikio Shimada Wood Research Institute, Kyoto University, Kyoto, Japan Kazumasa Shimizu Division of Wood Chemistry, Forestry and Forest Products Research Institute. Ibaraki, Japan Nobuo Shiraishi Division of Forest and Biomaterials Science. Graduatc riculture. Kyoto University, Kyoto. Japan
School of Ag-
Toshiaki Umezawa Wood Research Institute. Kyoto University, Kyoto. Japan Mariko Yoshioka Division of Forest and Biolnaterials Science, Graduate School of Agriculture, Kyoto University, Kyoto, Japan
Ultrastructure and Formation of Wood Cell Wall Minoru Fujita and Hiroshi Harada Kyoto University, Kyoto, Japan
1.
A.
GENERAL STRUCTURE OFWOOD AND WOOD CELLS Wood
SoftwoodandHardwood In introduction it should be understood that the term “wood” refers to the secondary xylem formed by cell division in the vascular cambium of both gymnosperms (softwoods) and angiosperms(hardwoods). and especially i n Ginkgo. Similarsecondary xylem may be produced by plants of different form and structure, such as vines and shrubs, the xylem of which may be an important resource of pulping material. The structure and formation of the secondary xylem are discussed in this chapter. Both softwoods and hardwoods are widely distributed on earth, from tropical to arctic regions.The xylem of those species present in moderate-temperate to arcticregions is characterized by distinct growth rings, in which some anatomical differences can be noted. In the softwoods consisting mainly of tracheids (approximately 90% of wood volume), the latewood (summer wood) can be distinguished from the earlywood (spring wood) by its smaller radial dimensions and thickercells walls. Theseanatomicaldifferenccsare reflected in the higher density of the latewood compared with the earlywood. In softwoods growing i n tropical or warm areas, growth rings cannot be distinguished due to the indistinct boundary between earlywood and latewood. As with the softwoods, hardwoods are also present i n tropical to arctic regions. In colderregions,hardwoodspeciesaredeciduous, whereas i n tropical regions, they are predominantly evergreen and their growth rings are difficult to recognize. The macroscopic characteristics of hardwoods are reflected in the distribution and number of different ccll typessuch as vessels (pores),parenchyma, and fibers. Although fibers may account for only 25% of wood volume, in some cases, for hardwood, it may be as high as 50-70%. In contrast to the tracheid as the main cell in softwoods,hardwoods have a variety of cells. Some deciduous hardwoods such a s oak or elm have very large vessels concentrated at the beginning of annual rings. Suchwoodsare called “ring porous wood,”whereas otherdeciduousspecies and almost all evergreen hardwoods in which the vesselsare evenly dispersed over the annual ring are callcd “diffuse porous wood.” The above dis1.
1
Harada 2
and
Fujita
tinctions represent extremes and there are many intermediate arrangements of the vessels. Variations in arrangements of these vessels with other xylem tissues such as parenchyma are reflected in the “figure” and “grain” of the wood itself when it is cut from the tree. The physical properties of wood such as density also result from such arrangements of the cells.
2. Sapwood and Heartwood When a tree stem is cut transversely, a portion of “heartwood” can be seen frequently as a dark-colored zone near the center of the stem. This portion is surrounded by a lightcolored peripheral zone called “sapwood.” The sapwood or at least the outer part of the stem conducts water throughthe tissue where the water is transpired, and mineral nutrients are also carried with water from the roots into the wood. In addition, the sapwood has living parenchyma tissue, which often plays some physiological role such as the storage of starch or fat. From this point of view, the sapwood is considered an active xylem tissue. In contrast to sapwood, heartwood is dead xylem. As the tree matures, all parenchyma cells of the sapwood die, and other typesof cells such as tracheids or fibers become occluded with pigment composed of polyphenols and flavanoids supplied mainly from the ray parenchyma. The bordered pits of gymnosperms become aspirated, whereas the vessels are blocked by tyloses or gum in angiosperms. Thus, heartwood does not participate in water conduction. Although the conducting and physiological functions are lost in heartwood. the durability of wood against rot or insect decay is remarkably improved due to an addition of such pigments. Moreover, these pigments confer a variety of beautiful colors on wood. 3. Reaction Wood Reaction woods that appear on branches or a leaning stem by any force such as a landslide or snowfall have a peculiar nature. Once reaction wood is formed as a biological response, the living tree tries topreserve the original position of its stemorbranches.For the practical use of woods, the reaction woods have not been appreciated very much because of their different characteristics fromnormalwood in both a physical and a chemical sense. The occurrence and nature of reaction woods contrast quite a bit between softwood and hardwood. In softwood trees, the reaction wood forms at the lower side of a leaning stem or branches, where the compression stress reacts on the xylem. Therefore, this reaction wood is generally called “compression wood.” compression woodis heavy and appears dark brown on account of its highly lignified tracheid walls (see Section II), which seem to adapt to compression stress. Thus, compression wood is easily distinguished from normal wood by its dark color. The cambial activity at the lower position of a leaning stemorbranchacceleratesveryquicklyanddevelops a widercompressionareathan normal wood on the opposite side. Through the accumulation of compression wood tracheids over many years, a leaning stem will return gradually to the vertical position. The annual rings of such a stem, however, are conspicuously eccentric. On the contrary, reaction wood in many species of hardwoods is formed at the upper side of a leaning stem or branches where the xylem loads the tensile stress. Therefore, such reaction woods are called “tension wood.” Fibers of tension wood have a slightly lignified cell wall (see Section 11) that is adapted to the tensile stress just like a bowstring. It is not so easy to distinguish this area from a normal one on account of its slightly pale tone, in comparison to the case of compression wood.
Formation Ultrastructure and
Wall
of Cell
3
In fact, the occurrence of both reaction woods is averytroublesomeproblem in wood utilization. These reaction woods, however, are interesting material for the examination of wood structure and formation, as will be noted often in the following sections.
B. Wood Cells Wood cells are produced in the vascular cambium from two types of meristematic cells: the fusiform initial and the ray initial (Fig. l ) . Since cells derived fromthe fusiform initials that are upright in the stem occupy a major part of xylem, woods show remarkable anisotropism. The principal functions of xylem tissue are water conduction from roots to shoots, the mechanical support of a huge tree body, and a physiological role such as the storage of starch. Although these functions are common in both softwoods and hardwoods, the xylem of the latter is more evolved than that of the former, being adapted to each function.
softwood
hardwood
pits
%I
fusiform initials
a
xial parenchyma cells
.B@'
ray tracheid FIGURE 1 hardwood.
axial parenchyma c e l l s
ray \ parenchyma ray cell initials p
Shapes of major wood cells fromthefusiformandrayinitialsinsoftwoodand
Harada 4
and
Fujita
I n softwoodsand Ginkgo, tracheids, beingmajorcells of xylem, are considered relatively underevolvedbecausetheyhavebothconductiveandmechanical properties. Bordered pits, the occurrence of which define a cell as a tracheid, are very important to the regulation of water flow. On the other hand, cell wall thickness is related directly to the strength of tracheids. The earlywood tracheids, therefore, seem to be well adapted to the conducting function whereas the latewood tracheids are loaded with the mechanical property, judging from their peculiar shapes. On the earlywood tracheids, well-developed pit pairs are distributed abundantly between the neighboring tracheids, and the cell walls of latewood tracheids are very thick. Only a small number of fusiform cells are subdivided into strand cells by horizontal partitions and compose an axial parenchyma. These parenchymatous cells survive in the sapwood for many years, being different from the tracheid, in which the protoplast is lost soon after differentiation (see Section III), and are part of some physiological functions. In somegenera of Pinaceae, axial resin canalssurrounded by epitherial cells are constructed. The occurrence and structure of resin canals are often used in the identification of softwoods, although the volume of such resin canals is very slight in wood. Ray cells are derived from the ray initials and elongated radially. A series of these ray cells make a ray parenchyma. Needless to say, these parenchyma cells are alive in the sapwood and are tied to the storage of nutrients such as starch or fat and also the transportation of some metabolites between the phloem and the heartwood. As a result, they must be related to the secretion of heartwood substance into the tracheids. Also, in some genera of Pinaceae, radial resin canals surrounded by epitherial cells are formed in many ray tissues, and more ray tracheids occur in the ray tissues. Hardwood xylem can be characterized by the development of vessel elements and wood fibers specialized for water conduction and the mechanical property, respectively. The vessel elements construct a very long and thick tube, namely, a vessel, being joined vertically with one another by a perforation that has a more developed style compared with the bordered pit pairs between tracheids. The occurrence of perforation distinguishes the vessel elements from the tracheids. Wood fibers elongate remarkably and possess very thick cell walls. The most developed type of cell, having simple pits (see Section II), is called libriform wood fiber. On the other hand, there are some intermediating cells from the tracheids to the vessel elements or wood fibers, i.e., vascular tracheids, vascentric tracheids, andfiber tracheids. The fiber tracheids are often included in the categoryof wood fibers. because there is no need to separate them from the libriform wood fibers in the practical use of wood. Vessel elements, wood fibers, and various types of tracheids in the hardwoods lose their protoplast just after the development of their secondary wall. However. in some hardwood species specialized wood fibers that remain alive for several years and often store starch grains are formed; they are called “living wood fibers.” Axial parenchyma cells, which are dispersed on the transverse section of softwoods, are clustered at the vessel periphery or form a group that is often linked tangentially. Resin canals that are surrounded by epitherial cells are formed in many genera of Dipterocarpaceae and a few Leguminosae. Ray parenchyma cells sometimes aggregate and develop a so-called broad ray. The broad rays make a peculiar figure on a board. especially on the radial surface, as observed in oak or beech. Cells contained i n the ray also vary in their anatomical features. Some of them are upright or square at the marginal position. These variations are used for the identitication of hardwoods [ l ] . Both axial and ray parenchyma cells are apparently concerned with physiological functions-for instance, the storage of nutrients or heartwood
Formation Ultrastructure and
Wall
of Cell
5
formation. Radial resin canals or latex tubes are formed in the ray tissue of some tropical hardwoods.
II.
ULTRASTRUCTURE OF WOOD CELL WALL
Wood is a natural composite material and a chemical complex of cellulose, lignin, hemicelluloses, and extractives [2]. Cellulose is the framework substance, comprising 40-50% of wood in the form of cellulose microfibrils, whereas hemicelluloses are the matrix substances present between cellulose microfibrils. Lignin, on the other hand, is the encrusting substance solidifying the cell wall associated with the matrix substances. The significance of lignin as the encrusting substance can be demonstrated by examination of the lignin skeleton created by the acid removal of carbohydrates (Fig. 2). The roles of these three chemical substances in the cell wall are compared to those of the constructing materials in the structures made from the reinforced concretein which cellulose, lignin, and hemicelluloses correspond, respectively, to the iron core, cement, and buffering material to improve their bonding.
A.
Cellulose Microfibrils
The crystalline nature of cellulose in wood has been demonstrated by studies with X-ray diffractometry and polarization microscopy. This crystalline nature was also confirmed by the electron diffraction patterns of the secondary walls of wood cells in selected areas [3]. Figure 3a isatransmissionelectronmicrograph of a longitudinalsection of latewood tracheids of Pinus densifloru, showing the intercellular layer (I), and the S, and S, layers. The electron diffraction diagram is of a selected area in S2 (Fig. 3b), which is represented by a small circle. The (101), (loi), and (002) of the equatorial reflections and (040) of
i
FIGURE 2 Electron micrograph of ultrathin transverse section of earlywood tracheids from Pinus densgora, showing thedistribution of lignin inthe cell wall, which was skeletonized using the hydrofluoric acid technique.
6
Fujita and Harada
FIGURE 3 (a) Electron micrograph of ultrathin longitudinal section of tension wood fibers from Pinus densiporu. (b) The corresponding diffraction diagram taken from the encircled area.
Formation Ultrastructure and
Wall
of Cell
7
the meridional reflection can be seen. It should be noted that crystallographic planes are based on the Meyer and Misch (1937) model of the unit cell of cellulose I, i n which the h axis (the fiber axis) is vertical. I t iswell known that in the wood cell wall, celluloseexists in the form ofthin threads with an indefinite length. Such threads are called cellulose microfibrils, and they play an important role in the chemical, physical, and mechanical properties of the wood. The greenalga, Kdorzia. which is oneform of Chlorophyceae,hasbeenstudied intensively by microscopists and crystallographers as an excellent material for the ultrastructural study of cellulose microfibril. Why then is W o t z i a used for the study of the cellulose microfibril of the wood cell wall? Because the cell walls of Valonia are unlignified, their microfibrils are readily isolated. Furthermore, as described later, Vrtlonicc microfibrils are approximately 20 nm in width, which is about five times larger than those of wood, and they are highly crystallized. However, the difference between algal microfibrils such as those of Vhlorli~zand ordinary ones produced by the higher plants also must be stressed. One of the differences is the selectively uniplaner orientation of algal microfibrils, that is, the ( 101) plane facing the cell surface, while cellulose microfibrils of higher plants are randomly oriented, although both microfibrils are laid along the cell surface i n their longitudinal direction [3,4]. The other is the crystallographic heterogeneity in algal microtibrils as detected by NMR [ S ] , and a triclinic system mixed with an ordinary monoclinic system was detected by electron diffraction [6]. The interface between these systems is not yet shown, although the former amounts to about 50%.
1. Dimensions of the Cellulose Microfibril As described above, it is clearly demonstrated through electron microscopy that the cellulose molecular chains are organized into strands as cellulose microfibrils. Figure 4 shows transmission electron micrographs of disintegrated cellulose microfibrils negatively stained withuranyl acetate. Figures .la and 4b, respectively, show the microfibrils of klonicr tnc~cmphyscrcell wall and the holocellulose of Pirlus drnsijur-a. A discrepancy in the size of the crystalline region of cellulose, obtained by X-ray diffractometry and electron microscopy, led to differing concepts as to the molecular organization of microfibrils. Frey-Wyssling 171 regarded the microfibril itself as being made up of a number of crystallites, each of which was separated by a paracrystalline region and later termed“elementary fibril” by Frey-WysslingandMuhlethaler 181. The term “elementary fibril” is therefore applied to the smallest cellulosic strand. Muhlethaler [ 10,l 11 applied this term to the cellulose fibril with a diameter of approximately 3.5 nm, using the negative-contrastpreparationtechnique for electron microscopy.Preston and Cronshaw [91,on the otherhand,considered the microfibril tohaveasinglecore of cellulose crystallite surrounded by a paracrystalline region. The width of cellulose microfibrils is reported to vary in different cellulose materials [ 121. For instance, as shown i n Fig. 4, Vrrlorzia cellulose microfibrils, being about 20 nm wide, are much larger than those of wood holocellulose. Shown in Table 1 are the crystallite size and microfibril width for several cellulose materials [ 131. The crystallite size was estimated with Scherrer’s equation at the reflection (002) or (101) of X-ray diffractometry, whereas the microfibril widthsweremeasured directly from the electron micrographs. The width range and mode width are also included in this table. It should be noted that the size of crystallites varies in different sources of cellulose materials, for results from both X-ray diffractometry and electron microscopy. According to Heyn [ 141, the negative stain can penetrate only the regions accessible to water. Thus, the translucent parts seen on the electron micrographs correspond to the
8
Fujita and Harada
FIGURE 4 Electron micrographs of the cellulose microfibrils of Vuloniu mucrophysa (a) and of Pinus densifloru holocellulose (b) (disintegration, negatively stained with uranyl acetate), showing the difference of cellulose microfibril width between wood and Vuloniu.
Formation Ultrastructure and
Wall
of Cell
9
TABLE 1 Crystallite Size and Microfibril Width
Crystallite Microfibril size"width Samples Pinus dens$ora
2.02 002)
-
Untreated 2.76Holocellulose
(2.5)b
Populus euramericana
4.1
layer Gelatinous Normal wood Valonia 15-30
(002)
2.2 (002) 14.3 11.9 (101)
(20.0)b
'Reflection examined. hModewldth. Source: Ref. 12.
crystalline regions of cellulose. Therefore, the difference in the microfibril width must be ascribed to that in the size of cellulose crystallites. In addition, the values obtained are not always equal to the 3.5 nm in elementary fibrils proposed by Muhlethaler [ l l ] .
2. Cross-Sectional View of Cellulose Microfibrils Figures 5a and 5b are similar electron micrographs of the ultrathin cross section of cellulose microfibrils from Valonia macrophysa and the gelatinous layer of Populus euramericana tension wood fiber. These were obtained by means of diffraction contrast in the bright-field mode foran epoxy resin-embedded section. This technique reveals a crystalline region as a dark zone dueto electron diffraction. Thus, cellulose microfibrils have a highly
FIGURE5 Electron micrograph of ultrathin transverse section of cellulose microfibrils (diffraction contrast in the bright field mode), showing their cross-sectional views: (a) from Valonia macrophysa; (b) from G layer of Populus eurarnericana.
Harada10
and
Fujlta
crystalline nature. It is interesting to note in Fig. 5a that a Vuloniu microfibril does not have any subunits corresponding to the elementary fibrils [13,17]. Additionally, cellulose microfibrils appear to be almost square in their cross section in both wood and Vuloniu [15-171.
3. Crystalline Structure of Cellulose Microfibrils Figure6shows Vuloniu macrophysu microfibrilsmechanicallydisintegratedwithacid, taken by diffraction contrast in the bright-field mode. Cellulose microfibrils can be seen as the dark areas, again indicating the highly crystalline structureof cellulose. However, the internal crystalline ultrastructure of cellulose microfibrils is not revealed by electron microscopic techniques such as negative staining and diffraction contrast, because lattice imagesof cellulose microfibrils are not obtained. The most important reason is that cellulose microfibrils are damaged by the electron beam and their crystalline nature is destroyed by irradiation under normal photographing conditions. Recently, the crystalline ultrastructure of cellulose microfibrils in Vuloniu macroby a specially developed technique for taking highphysu cell wall has been revealed resolution lattice images [15,16]. Figure 7 is an example of the lattice fringe substructures from disintegrated cellulose microfibrils. This micrograph shows the lattice image of 0.60 nm, corresponding to thatof the (101) plane. The lattice spacingof 0.60 nm is also shown in the electron and optical diffraction patterns. The lattice lines are observed regularly at about 20 nm width across the cellulose microfibril and are also visible along its length for more than 50 nm without any disruption. Figure 8 shows images of the cross section of cellulose microfibrils obtained using ultrathin sections. Lattice lines at0.60, 0.54, and 0.39 nm are visible in this figure. Therefore, a single microfibril is indicated as the individual crystal. Accordingly, it is suggested that the crystal line subunits as 3.5 nm elementary fibril and periodicity in its length does not exist inside the cellulosemicrofibril. Unfortunately, lattice images of cellulose microfibrils have not yet been taken in wood cellulose, since wood cellulose has low crystallinity and the size of the cellulose
FIGURE6 Electron micrograph of cellulose microfibrils fromVuloniu mucrophysu (disintegration, diffraction contrast in the bright-field mode), showing the crystalline nature of cellulose microfibrils.
Formation Ultrastructure and
Wall
of Cell
11
FIGURE 7 Lattice image of a disintegrated cellulose microfibril of Valonia mcrophysa, showing the lattice spacing of 0.60 nm.
FIGURE 8 Lattice images of the cross-sectional face of cellulose microfibrils from Valonia macrophysa, showing the lattice spacings of 0.60, 0.54, and 0.39 nm, respectively.
Fujita and Harada
12
microfibril is rather smaller compared with that of Valonia. In the near future, beam damage at room temperature against wood cellulose microfibrils would be reduced at least 10 times with cryo-electron microscopy. The cellulose microfibrils of the gelatinous layer of poplar (Populus eurntnictrna) tension wood in disintegrated samples are found to have many kinks, suggesting that the cellulose microfibril is highly crystalline [13]. However, the cellulose microfibrils of the gelatinous layer, about 100 nm in length prepared by ultramicrotome, become shorter than their original length upon hydrolysis [ 131. As a result, the crystalline regions in the cellulose microfibril of wood cell wall are thought to havesomecrystallinedislocations caused by chain ends [ 181. The cellulose microfibrils consist of a core crystalline region of cellulose surrounded by paracrystalline cellulose and short-chain hemicellulose. Lignin encases them and binds them into a rigid structure of wood cell wall.
B. Cell Wall Layers and Lamellae At the first step of differentiation of a woody cell, the living protoplasm produces a primary wall (P) that can be extensively increased in its surface as the cell develops. The substance between the primary walls of adjacent cells is called the intercellular layer (I) or the middle lamella. Since it is difficult to distinguish the region between the I layer and the P wall in the mature cell wall, the termcompoundmiddlelamella (CM) is generally used to designate the combined I layer and the two adjacent P walls. After the enlargement of the cell ceases. the cell wall layers are formed by the apposition of wall substances onto the inside of the primary wall. These wall layers are called the secondary wall (S) Although the primary wall andsecondarywallare classified by the ontogenetic process of plant cells, actual layered structures have been examined by the orientation of cellulose microfibrils. As a result the concept of lamellae, which are composed ofvery thin layers of only one or two cellulose microfibril width, is introduced. Cell walls were thickened by the appositional supply of these lamellae from the protoplast, so cellulosic interlamellae bridges are not accepted in the concept. The lamnella structure on the secondary wall is interesting in both physical and chemical properties of wood. Kerrer and Goring proposed a composite model with hemicelluloses and lignin [IS]. Although it is very intelligent, actual microfibril orientation on a lamella may fluctuate more [2O,2 I ] .
1.
Tracheids and Fibers
Figures 9 and I O are polarized photomicrographs at crosscd polars of transverse sections of tracheids and fibers, respectively. Both reveal the three-layered structure of the cell wall due to the differences in the orientation of cellulose microfibrils. According to the concept of Kerr and Bailey [22], normal wood cell wall consists of P and S walls, and the S wall is composed of a relatively narrowor thin outer layer (S,), an inner layer (S3), and a relatively thick middle layer (S?). However, the P wall cannot be distinguished in the figure due to the strong birefringence of the S , layer adjacent to the P wall. The S , and S, layers appear bright in the photographs, whereas the S, layer is at total extinction. That the birefringence of the S, layer occurs to a lesser degree than that of S , in the fibers of F q u s crewtcl indicates the poordevelopment of the S,. Despitesubsequentextensive studies with electron microscopy, the concept and terminology described above are still commonly accepted. Figure 1 1 is an electron micrograph ofan ultrathin transverse section from Cty7tomer-iajapotzicn, stained with silver protenate. It shows the intercellular layer (I), different
Ultrastructureand Formationof Cell Wall
13
I
FIGURE 9 Polarized-lightphotomicrograph of transverse section from earlywood tracheids of Pinus c/ensiforu, showing thethree-layeredstructure of the cell wall due to the birefringence of cellulose microfibrils.
layers of the secondary wall (S), and the warty layer (W) in an earlywood tracheid. The same layering structure from an earlywood tracheid of Pinus densiflot-a is shown more clearly in a longitudinal section that was skeletonized by the hydrofluoric acid technique (Fig. 12). Figure 16, (pg. 18). shows the texture of the P wall diagrammatically. The microfibril orientation in the primary wall was interpreted by the multinet growth hypothesis proposed by Roelofsen [23] and supported for the differentiating conifer tracheids by Wardrop[24].
FIGURE 10 Polarized-lightphotomicrograph of transverse section from wood fibers of Fugus crenatcr, showing the same structures as in Fig. 9.
14
Fujita and Harada
FIGURE 11 Electronmicrograph of ultrathintransverse section of an earlywood tracheidfrom Cryptomeria japonica, showing I, S,, S*, S1,and W (warty layer) at the final differentiating stage of the cell wall.
FIGURE 12 Electronmicrograph of ultrathinlongitudinal section of earlywood tracheidsfrom Pinus densifom (skeletonized cell wall with the hydrofluoric acid method), showing the I, P, S,, Sl, and S3 of the cell wall.
Formation Ultrastructure and
Wall of Cell
15
In the multinet hypothesis, the microfibrils are first deposited transversely to the cell axis and passively shifted longitudinally during cell extension. From an opposite viewpoint, an orderedfibrilhypothesiswasproposed by Roland et al. [25] in order to interpret the crossed polylamellated structure in the primary wall of parenchyma cells. According to this hypothesis, whether the orientation of microfibrils becomes transverse, oblique, or longitudinal is determined at the time of deposition of cell wall and may not be changed thereafter. Recently, Fujii et al. [26] proposed a modified multinet hypothesis of microfibrils orientation in the primary wall. The difference between this conceptand Roelofsen’s theoryisthattheshift of microfibrilorientation during cell extension is made in the individual lamella and each lamella becomes thin on the outer surface of the P wall due to extension. The three layers of the secondary wall, designated S,,S2, and S3,are organized in a plywood type of construction. The S , or S3,with a large microfibril angle to the cell axis, is designated as a flat helix, and the S2,with a small angle, as a steep helix (see Fig. 16). It is also shown that the layers themselves are of lamellae of microfibrils with varying amounts of shift in orientation, visible in the transmission electron micrograph. The S , is composed of several lamellae with alternating S and Z helices of microfibril orientation [28,29], and this structure in the S , is termed “crossed fibrilar texture” [28]. Figure 13 is
FIGURE 13 Electronmicrograph of theradialinnersurfacein a differentiatingtracheidfrom Pirzus densgoru (direct carbon replica), showing the microfibrillar orientation of the newly deposited microlamella crossing that of the underlying microlamella in S,.
Harada16
and
Fujita
a transmission electron micrograph of a replica of the inner surface of the differentiating early wood tracheid of Pinus densgora forming the S,, showing the criss-crossed texture of the microfibril orientation in the two different lamellae. The middle layer of the secondary wall (S,) is the thickest within the layers of the secondary wall. Therefore, the S, contributes most to the bulk of the cell wall material and is a compact region in which a high degree of parallelism of microfibrils exists. The S, isathinlayer of flathelices of microfibrilorientationasseenin S,. As opposed to the highly oriented S,, the S, is loosely textured. The S,, birefringent to a somewhat lesser degree than theS, in wood fiber, shows that this layer is poorly developed. Althoughthe S2 exhibitsamicrofibrillarorientationwithsteephelices,there are transition lamellae on its inner and outer surfaces. Several lamellae in these regions show agradualshift of microfibrilanglesbetween S, and S, andbetween S, and SJ [30]. However, the gradual shift of microfibril angles is more abrupt between S, and S, than between S, and S,. The transition lamellae in the secondary wall are not detected in TEM micrographs of ultrathin sections, since this lamella is relatively thin compared with the S, and S,. The method for evaluating microfibril angles in the secondary wall of wood cells was proposed by Yamanaka [31]. Figure 14 is a "EM micrograph of a transversely oblique section of an earlywood tracheid from Pinus dens.ijZora (stained with KMnO,). The curve through black dots shows the changes of the microfibrillar angle with respect
F FIGURE 14 Electron micrograph of ultrathin oblique section of an earlywood tracheid in Pinus densijffloraand microfibril angles in the secondary wall: top, I. bottom, lumen side.
Formation Ultrastructure and
of Cell Wall
17
to the tracheid axis from the top S, to the bottom S,. The horizontal line in the upper part of the figure shows the angles of microfibrillar orientation, the symbols (-) and (+), respectively, referring to Z and S helices. The gradual changes of the microfibrillar angles from S, to S, and from S, to S, are shown there. The helical cellulose microfibril orientationin the S, is typically demonstrated in Xray diagrams of wood [32]. The arcs at 0.39, 0.54, and 0.60 nm in the X-ray diagram of wood show that the cellulose crystallites (microfibrils) lie in a helix around each wood fiber or tracheid. The microfibril orientations are Z helices in the S, and S helices in the S,, although S, is the crossed arrangement of S and Z helices. Preston [32] suggests that the structure with various microfibril angles in the secondary wall passes through only one cycle, but this may be the brief duration of wall thickening in higher-plant cell walls compared with that in algae. Roland and Mosiniak [33] presented a diagram regarding the changesof cellulose microfibril angles in the case of a secondary wall of tracheids and wood fibers (Fig. 15). Figure 15 illustrates the case between the S, and S, layer. The change of microfibril angle is regular and continuous between the S , and S, layers,butitstopsduringthe deposition of the S , layer. Afterwards the change of microfibril angle reopens toward S, layer deposition. The texture of cellulose microfibrils in the P and S walls of softwood tracheids and hardwood fibers is shown as a schematic diagram in Fig. 16. The thin primary wall (P) consists of a loose aggregation of microfibrils oriented more or less axially to the cell axis on the outer surface. The S, layer is a flat helix but with crossed structure, whereas the S, layer is a steep helix and the S, layer is a flat helix. There are intermediate layers: the S,,, present between the S , and S, layers; and the S,,, between the S, and S, layers. The spiral thickening is the ridge of microfibrils that exist on the inner surface of the S, layer. The spiral thickening is considered part of the S, layer becauseof its continuity with the S, layer and parallel arrangement to the S, layer microfibrils.
FIGURE 15 Schematic diagram of the change of microfibrilorientationfrom three-layered structure of the cell wall. (From Ref. 32.)
S, and Sz in the
Harada18
and
FuJlta
FIGURE 16 Schematic diagram of the microfibril orientation in the primary wall and different layers of the secondary wall from tracheids and fibers: Po,PI;outer and inner parts of the primary wall; SlzrS23, intermediate layers between S , and S , and between S2 and S,, respectively.
The warty layer is one of the major structural features of wood cells found by electron microscopy [34]. It was first foundin softwood tracheids and laterin the tracheids, vessels, and wood fibers of hardwoods (see Fig. 11). The major chemical constituents of warts arereported to be lignin and hemicelluloses according to examination by component removal treatment of ultrathin wood sections [35]. The warts are believed to arise from the extra wall materials and remains of cytoplasm that are deposited on the S, layer through the plasma membrane [36,37]. The warty layer is not found in all softwoods and hardwoods [30,38]. Parham and Baird [39] have pointed out that the appearance of warts in wood has a phylogenetic trend. Softwood tracheids and primitive hardwood cells nearly always have warts, but as the cell types become more advanced or specialized, they become wart-free.
2. Vessels The texture of cellulose microfibrils in the walls of specialized cells such as vessel elements and parenchyma cells cannot be readily described as in softwood tracheids and hardwood fibers. A concept of standardized cell wall organization in vessel elements was, however, represented by Kishi et al. [40,41]. The microfibrils in the primary wall extend straight and are arranged parallel to one another within one lamella, and the wall consists of three parts, P-outer, P-middle, and P-inner, each showing a different microfibril orientation. The microfibrils are oriented transversely with respect to the vessel axis in the Pouter and are oriented at random in the P-middle. The P-inner consists of a crossed polylamellatedstructure. It isalsoreportedfromthe examination of vessel elements from nearly 30 Japanese hardwoods with polarizing and electron microscopy that the layered structure of the secondary wall can be classified into three categories: the typical threelayered structure, an unlayered structure, and a multilayered structure. The typical threelayered structure consists of S,, S2,and S3 similar to those of softwood tracheids and hardwood fibers, although the S, and S3 layers are thicker than those of tracheids and
Formation Ultrastructure and
Wall of Cell
19
wood fibers. The unlayered structure has only microfibrils, with the orientation of a flat helix. The multilayered structure has more than four layers, in which microfibril angles to the vessel axis change. This type of structure contains in some cases the so-called bowshaped pattern. Figure 17 isa TEM micrograph of the transverse sectionof Cinnamomum camphora and shows the microfibril angle and helix in the part of the bow-shaped pattern appearing on the vessel wall of the multilayered type of structure. As shown in Fig. 17, the pattern results from the progressive changes of microfibrillar orientation in the wall from 90" to 0" and from 0" to 90".
3. Parenchyma Cells In spite of the fact that parenchyma cells had been generally considered to have only primary wall, thoseof wood are reported sometimes to develop secondary wall, in addition to complicated primary wall. It is evident from recent studies that ray and axial parenchyma cells in both softwoods and hardwoods have variations or complexities in their wall structure that are not observed in the cell walls of tracheids and wood fibers. In softwoods, the cell wall structure of the ray parenchyma cells was divided into five categories by Fujikawa and Ishida [42]. However, as shown in Fig. 18, it is fundamentally classified into two types; the firsttype consists of the primary walland protective
b
90 FIGURE 17 Electron micrograph of ultrathin oblique sectionof a vessel wall stained withKMnO., from Cinnamomum camphora, showing a bow-shaped pattern (a) and the microfibril angles and helices (b).
20
Fujita and Harada
L-
i
I l
I I
P
S1
i
S2
1
I
FIGURE 18 Schematicdiagram of themicrofibrilorientation in the cell wall of softwood ray parenchyma cell: (a) the first type; (b) the second type. (From Ref. 41.)
layer (Fig. 18a), and the second type consists of the primary wall, secondary wall, and protective layer (Fig. 18b) [42]. However, the protective layer and a random arrangement of microfibrils is omitted in this figure. The P, appears with microfibrils of almost parallel orientation to the ray cell axis, the P, with the network appearance of microfibrils, and the P3 with several crossed polylamellate at microfibrillar angles of 30-60". It is interesting to note that the ray parenchymacell wall in thediploxylem of Pinus develops in two stages: that is, the primary wall and inner protective layer are fornled in the sapwood, and just before the heartwood is developed, the secondary wall and protective layer are deposited. In the axial parenchyma cells of softwood, the cell wall texture is very similar to that of ray parenchyma cells, except that the microfibrils are arranged in a flat helix with respect to the cell axis in the P , . In hardwoods, the primary wall ofray parenchyma cells has the so-called polylamellated structure proposed by Chafe and Chauret 1431. It was pointed out by Chafe and Chauret [43] that an isotropic layer and protective layer characterize the layered structure of the secondary wall of xylem parenchyma cells in hardwoods. According to examinations of thechemicalcomponents of these two layers using aseries of treatments on serial ultrathin sections, both a protective layer and an isotropic layer are rich in hemicelluloses and contain some pectic substances and cellulose microfibrils, but they have little lignin at the first stage of their developing process and become lignin-rich after the deposition of the inner secondary walls on them [44]. Consequently, both layers are considered the
Ultrastructureand Formation Wall of Cell
21
same in their origin and are called “amorphous layer” by Fujii et al. [M].Figure 19 shows electron micrographs of transverse sections by ray parenchyma cell from Tiliu juponicu; Fig. 19a shows cell walls skeletonized with hydrofluoric acid, while Fig. 19b shows sodiumchloride-treatedcellwalls.Blackzonesshow an amorphous layer indicating the presence of much lignin (Fig. 19a), but these disappear through delignification as seen in Fig.19b. It has been reportedbyFujii et al. [45] fromtheexamination of ray and axial parenchyma cell walls from about 50 species of Japanese hardwoods that the secondary wall is composed of a lignified cellulosic layer (CL) and an amorphous layer (AL) and that the cell wall structure can be classified into three types according to the presenceand organization of these two kinds of layers. Figure 20 is a schematic diagram of the cell wall organization of hardwood ray parenchyma cells: (1) 3CL-type, (2) 3CL+AL-type, (3) 3CL+AL+IL-type. CL refers to the lignified cellulosic layer that is similar to the ordinary wood cell wall, whereas ICL refers to the lignified cellulosic layer inside the amorphous layer (AL). The 3CL-type wall structuremay be considered thestandard structure of parenchyma cells of hardwoods, whereas the 3CL+AL-type wall structure occurs in cells that have extensive pit contact with vessels.
FIGURE 19 Electron micrographs of ultrathin cross section of the ray parenchyma cell from Tilia japonica, showing the amorphous layer (AL) of the secondary wall: (a) delignified cell wall; (b) cell wall skeletonized using hydrofluoric acid treatment.
Harada22
and 3CL
1-q
AL
Fujita
ICL
.: .............,..,..........:..-
x:
(a)
(C)
FIGURE 20 Schematic diagram of the cell wall organization of hardwood ray parenchyma cell, showing three types of wall structure: (a) 3CL; (b) 3CL AL,(c) 3CL + AL ICL.
+
4.
+
Reaction Wood Cell Wall
As described above (see Section I), softwood reaction wood is called compression wood and hardwood reaction wood is called tension wood. Figure 21 is a polarizing micrograph of compression wood tracheids from Pinus densijlora, and it demonstratesthat the S, layer present in normal wood tracheids is lacking. This is clearly shown in an electron micrograph of a cross section of a compression wood tracheid from Pinus densijioru (Fig. 22), and the presence of deep spiral checks in the S, layer is also revealed. The microfibrillar orientation of the S, layer is nearly 45",
Harada24
and
Fujita
cellulose of the G layer is highly crystalline. Its microfibrils are oriented parallel to the longitudinal axis of the fiber and the G layer is easily separated from the remainderof the fiber wall. Another structural feature of the tension wood fiber wall is that the G layer deposits on any one of the normal three secondary wall layers, S,, S2,and S,. The secondary wall of the tension wood fiber consists of three types, that is, S, G , S, S, G , and S, Sz + S, + G, depending on the wood species or part within a stem. Consequently, the G layer is called “the S, layer” when we refer to the S,, Sz,and S, layers.
+
C.
+
+
+
Sculpturing of the Wood Cell Wall
Cellulosic fibers such as cotton, ramie,and jute are relatively simple, smooth-walled composites of lamellae, but in wood the cell walls are almost invariably interrupted by gaps (pits) and sculpturing features.
1. Pit Structure Pits are gaps in the secondary wall of wood cells. There are two types of pits: bordered pits and simple pits. Generally, pits are present as pairs between two adjacent cells: bordered pit pairs, simple, and half-bordered pit pairs. In softwood, the pit border region of the cell wall is composed of border thickening (BT), S,, S2,and S, from the outer part of the cell wall as shown in Fig. 24. The presence of BT and thicker S, are features of the pit border wall. The microfibrils circle at theBT and sweep around thepit at the individual layers S,, Sz,and S,. In softwood bordered pit pairs, many species show a thickening at the center of the pit membrane. The torusis suspended from fine cellulosic strands to form a margin around the torus as shown in Fig. 25. The margin consists of an open net of
FIGURE 24 Schematic diagram of pit border organization in bordered pits of softwood tracheids. BT, initial pit border.
Formation Ultrastructure and
of Cell Wall
25
FIGURE 25 Electronmicrograph of the surface of pitmembranefrom Cryptomeria japonica (direct carbon replica), showing the pit membrane structure. T, torus; M, margo.
radially oriented microfibrils superimposed on an unoriented primary wall network, and it extends from the torus to the pit border. The torus is generally convex lens-shaped in cross section. On the other hand, the torus is seldom thickened in other cases. The former is true in species of the Pinaceae and Sciadopityaceae families, and the latter case involves species of Ginkgoaceae, Taxaceae, Chephalotaxaceae, Cupressaceae, Podocarpaceae, and Araucariaceae. The pit membrane of a half-bordered pit pair between tracheids and ray or axial parenchyma cells is quite thick. There is no torus in the center of the pit membrane, and no openings can be seen even at high magnification with an electron microscope. The central feature of the membrane structure of simple pit pairs in the interparenchymatous pits is the presence of plasmodesmatal pores. In hardwoods, the cell wallof the pit border consists of BT, P, S,, S*, and S3in tracheids and fiber tracheids of hardwood, like softwood tracheids. However, the pit border of vessels lacks not only BT but also S, in some parts of the pit border region [47]. The pit membrane of the bordered,half-bordered, and simple pit pairs in hardwoods is equal in thickness, exhibiting the primarywall texture, and there is usually no evidence of a torus. However, the presence of a torus in the intervessel pit membrane is reported in several species of hardwoods [48]. The pit membrane of simple pit pairs has plasmodesmatal pores as seen in softwoods.
Fujita and Harada
26
2. Vesture Pits In hardwoods, the pit chamber and pit apertures that are decorated by outgrowths of wall material are known as vestured pits. The outer growths of vestured pits are constructed chemically of lignin, hemicelluloses, and a little pectin [35].The shape and size of the outgrowths of vestured pits are variable. The development of vestured pit outgrowths is regarded as similar to that of warts. 111.
GENERAL DEVELOPMENT OF WOOD AND WOOD CELLS
A.
Vascular Cambium and Cambial Activity
One of the characteristic features ofa tree is the formationof the vascularcambium cylindrically surroundingastem,branches,and roots. The vascularcambiumproduces xylem inward and phloem outward. This sequence allows a tree to make itself a huge body. The cylindrical vascular cambium occurs through a series of developing meristem, namely, the apical meristem, the occurrence of procambium in the ground meristem, the growth of the vascular bundle, and the connection of intrafasicular cambium by the development of interfasicular cambium. The vascular cambium is composed of two types of meristematic cells. One is the fusiform initial occupying the major part of meristematic cells, and the other is the ray initial. Through their active cell division, parts of xylem and phloem are produced. However, since their activity in cell division is to a great extent affected by the season and weather, the result is the formation of annual rings in temperate regions. These initials must also multiply themselves on the tangential plane according to the increment of stem diameter. These two types of cell divisions can be distinguished by the direction of the division. The former division is defined as “periclinal division,” and the latter is called “anticlinal division” (see Figs. 26 and 27). Periclinal division is the mostimportant in view of woodformationandthus is discussed in detail. Cell division of the initial is extremelyrapid in spring. Moreover, several derivative cells (xylem mother cells) just inside the initial also have the ability to multiply through periclinal division. It is practically impossible to determine the true initial cell among these dividing cells. Therefore, just for convenience, a group of these cells is consideredcambialcellsand their area is called the cambialzone. In softwoods, the fusiform cells derived from the cambial zone differentiate directly into the tracheids except in onlyafewcasesinvolving the formation of the parenchymastrand,whereasthey differentiate into vessel elements, wood fibers, and several types of tracheids and parenchyma cells in hardwoods. Carnbial activity and the derivative differentiation are very important sequences in the growth of trees, environmental preservation of forests, and production of wood as a biomaterial. That is, they are the major sink of organic substances which are synthesized on leaves by CO, fixation, and then the major source of other life activities such as insects and also human beings. A detailed review of the vascular cambium has been published by Larson [491.
B.
Differentiation of Wood Cells
The tern1 “differentiation” has several meanings in the fieldof biology. I n this chapter, the term will be applied to the restricted case of the process of cell devclopment from the just-forming state i n the meristematic tissue to the mature state at which it is accomplished.
P
..
R.
l!
I f
FIGURE 26 (a) Light micrograph around the cambial zone ( C ) ,phloem (Ph), and enlarging xylem (E) from a transverse section of Robinia pseudoacacia. Most fusiform cambial cells are undergoing periclinal division, except for a trace experiencing anticlinal division (arrow).(b) Electron micrograph of fusiform and ray cambial cells. (c) Cytoplasmic feature of enlarging cells. 27
28
Fujlta and Harada
FIGURE 26 Continued
For instance, the differentiation of tracheids implies their maturing process from birth at the cambial zone to death after the secondary wall formation, by which both water-conducting functions and mechanical properties are given to the tracheid. The method of differentiation of parenchyma cells is quite different from that of tracheids, because they have only the primary wall or an underdeveloped secondary wall on the primary wall. They may be already functioning at thecambial zoneand have the ability to redifferentiate. Therefore, their differentiation is not addressed here. First of all, the differentiationof softwood tracheids, which is the most basic process of wood cell formation, will be discussed in detail. When a specimen block around the cambial zone is taken from the stem of a living tree and then a transverse section is observed under a light microscope, it is noticed that cells are piling up on a radial row from the mature phloem to the mature xylem through the cambial zone (Fig. 27a). The differentiating zoneof tracheids is located between the cambial zone and the mature xylem area. If the whole life of a particular tracheid from birth to death could be traced in situ in a tree stem, the tracheid differentiation would be clearly elucidated. However, it is really impossible to do so because the cells must be fixed with some reagent to preserve their cytoplasmic structure. Regrettably, their dynamic cell actions evolve into static phase by fixation. Therefore, the differentiating process of a tracheid must be deduced from the static cell structure of a series of differentiating tracheids. From this point of view, the differentiating zone of earlywood tracheids is favored for the precise examinationof their differentiation. In the spring, the production of tracheids from the cambial zone is very
D
3
Q
n 0
7
3
s
0
3
FIGURE 27 (a) Light micrograph of the cambial zone (C) and the derivative tracheids in five differentiating stages (RE, S,, S,, S3, and F) between phloem (Ph) and mature xylem (MX)from Cryprorneriujuponicu. (b) Enlarged view of S, depositing cells.
h)
W
Harada30
and
Fujlta
FIGURE 27 Continued
constant and, as a result, a series of differentiating tracheids is lined up in an orderly fashion along a radialrow from the just-formed stage to the mature stage. This series can be considered a good substitute for the life story of a tracheid, and since it is possible to trace the series using many microscopic techniques, the differentiating processof a tracheid can be grasped dynamically by tracing these differentiating tracheids along radial rows (Fig. 27a). Thedifferentiation of tracheids will be separatedintoseveral developing stages. Tracheids are pushed out in an inward direction from the cambial zone so as to begin enlargement. In the case of tracheids, the enlargement proceeds mainly in the radial direction, whereas enlargement in the tangential and longitudinal directions is very slight. Therefore, it may be appropriate to call this stage the radial enlarging (RE) stage. This fact results in the thinner radial walls of tracheids and the reorientation of cellulose microfibrils that may occur during the extension of the wall. The tracheid in this stage is composed of primary wall similar to the wallof cambial stage (C) cells. The thinned wall is recovered by the supplement of new wall materials on the inner surface. The extended wall is so fragile that it is often damaged and tom off during sampling of a specimen block from a living stem. After the enlargement of cell size, tracheids thicken secondary wall layers with the formation of the S,, S?, and S, layers. These stages are performed by the active deposition of cellulose microfibrils. However, the outermost region of the cell wall, including the intercellular layer, the cell comers, and the primary wall, is lignified during the S, stage. This lignification, which will be called “intercellular layer W i g n i fication,” may play an important role in stabilizing the cell size and conjugating the differentiating cells with one another. This I-lignification is accomplished in the middle phase of the S2 stage. Hemicelluloses are also supplied just after the deposition of cellulose
Formation Ultrastructure and
of Cell Wall
31
microfibrils (see Section IV). The secondary wall, which is still porous and flexible after the deposition of hemicelluloses, is encrusted with lignin and becomes very rigid. The lignification of the secondary wall, which willbe called “S-lignification” in contrast to “I-lignification,” is the most active after the S, stage,namely, in thefinal (F) stage of differentiation, although its initiation can be detected already during the S, stage. In this F stage some decorative elements such as warts or helical thickenings are added on the inner surface of the wall. After the wall layers develop, tracheids lose their cytoplasm by autolysis. Amorphous substances that have embedded the pit membrane also dissolve enzymatically sometime in the F stage. Tracheid differentiation is completed as this point and water conduction is achieved in the mature xylem (MX). The differentiation of vessel elements is characterized by enormousexpansion in both the radial and tangential directions. Although the developing stages of tracheids cannotbe applied directly to those of vessel elementsdue to a different secondary wall structure, the relationship of enlargement to secondary wall thickening and lignification is consideredsimilar to the sequence of tracheid differentiation. Needless to say, the formation of perforation pores is completed by the disappearance of the membrane itself, apart from the removal of only an embedding substance in the bordered pit pairs. On the contrary, the differentiation of wood fibers is characterized by the remarkable elongation in cell length that occurs at cell tips [50], and the other properties of differentiation are quite similar to those of tracheids. In hardwood, although the differentiation of both vessel elements and wood fibers proceeds simultaneously, vessel elements differentiate faster than wood fibers. How long a wood cell needs for its differentiation is also an important question. The time requirement for differentiation has been deduced by several methods, but the results are conflicting. A detailed timerequirementwascalculated for young trees of several softwoods by means of periodic inclinations for the internal date marking on the xylem. By these markings and the cell numbers contained in each differentiating stage, a time requirementofabout three weeks for passingthrough the five developingstages of a tracheid (RE, S , , S?, S,, and F) was calculated [51].
C. Cytology of Wood Cells Cambial cells, the differentiating cells of the tracheid, vessel element, and wood fiber, and also living parenchyma cells possess protoplast in their cell lumens. The most peculiar cytoplasmic structure of the fusiformcambialcells is the existence of ahuge central vacuole (CV) (Fig. 26b). This vacuole is maintained during the differentiation of tracheids (Fig. 27b), vessel elements,and wood fibers, whereas the cytoplasmicregion(Cy) is restricted to the very narrow area between the plasma membrane (Pm) and the vacuole membrane tonoplast (T) (Fig. 26c). On the contrary, the ray cambial cells and their derivative parenchyma cells are full of cytoplasm in their cell lumen, although several smaller vacuoles sometimes occur (Fig. 26b). In the axial parenchyma cells formed by the redivision of a young fusiform derivative, the central vacuole becomes small, and the cytoplasmic area expands in the reverse way. In spite of the cambial zone and differentiating xylem existing under the circumstance of very high pressure between the bark and mature xylem, the cellscontained in this areahaveonlya thin wall. Althoughvacuolation is generally considered a symptom of cell decay, the conspicuous vacuolation of these cells is supposedtoplay a very important role in the sustainment of their cell shapeunder presure. The enlargement of cell volume also depends on the turgor pressure of the vac-
32
Fujita and Harada
uole. In fact, it can be pointed out by arealneasurements that the vacuole is the best developed of the cells at the RE stage, when cells are just expanding (Fig. 28a). A nucleous is located around the central position of a fusiform cell in the longitudinal direction [SO], but on the transverse plane it is still pushed to one side of the cell lumen by vacuolation (Fig. 26c). In the cytoplasm, ordinary cell organelles such as Golgi bodies (Go),rough and smooth endoplasmic reticula (r-ER and S-ER). mitochondria (M), plastids (P), small vesicles (v), ribosomes, microtubules, and so on, are contained in a very narrow cytoplasmic region, although the occurrence of these cell organelles except microtubules between plasma membrane (Pm) and tonoplast (T) is not so abundant during the difl’erentiation of tracheids, wood tibers, or vessel elements. On the contrary, the cytoplasm of differentiating ray and axial parenchyma cells is crowded with many cell organelles. Especially, starch grains in the plastids and lipid droplets are very abundant, and r-ER are also well developed, whereas microtubules are very scarce. Ray cambial cells and mature ray cells arc almost identical to the differentiating parenchyma cells in their cytoplasmic features(Fig.26b). However, the number and size of starchgrains and lipid droplets contained in mature parenchyma cells change during a year 152-541. Thecytoplasmicfeatures of tracheidschange 21 little both i n quality and quantity according to their differentiation. The increase and decrease of the cytoplasmic area and its constituents of cell organelles were revealed by the combined use of light microscopy (Fig. 28a) and electron microscopy (Fig. 2%) on the differentiating zones of normal and compression woods of Cqptmtwricr juponicu. Areas of cell outline (A,,,,,,,;,,),cytoplasmicsurface (A,,,,,,,,,),and central vacuole (A,,,,,,,,,) were measured on an enlarged light micrograph of the transversesections o f differentiating tracheids using a digitized system connected to a computer (Fig. 28a). The nxasuretnent was performedalongthedifferentiatingtracheids, which were numbered from the initiation of the S , stage, and about 30 radial rows were surveyed. These radial rows of tracheids were sectioned at random in their longitudinal direction, so that the average value of tracheids of the same cell number reflects the makeup of volume i n each region. Areas of cell wall (A,v,J and cytoplasm (A,,.,,,,,,,,,,,) can be calculated by finding the remainder between those of the cell outline, the cytoplasmic surface. and the central vacuole, respectively. These values are diagramed in Figs. 29 and 30. I t should be noted that the cytoplasmic volume of both the normal and compression woods has two peaks during tracheid differentiation. The earlier peak i n both cases is at the intermediating phase from the S , stage to the S, stage, whereas the later one is located just prior to the initiation of the S , or F stage. On the contrary, during the S2 thickening, the cytoplasm is rather poor. Following this, proportions i n RE, S , , early S?, middle S,, late S,, and S, stages (Fig. 29) show the relative constituents of major cell organelles surveyed by electron microscopy (Fig. 2%). The general change in these cell organelles can be grasped by inultiplying the relative value by the total area of cytoplasm diagramed in Fig. 29. In addition to the changes in these cell organelles, the plasma membrane, important to the transportation of materials in and out of the cytoplasm, is always observed during tracheid differentiation and disappears after the development of the cell wall. The cytoplasmic features of differentiating wood fibers and vessel elements are also similar to those of tracheid differentiation, although the vacuolation of vessel elements is Inore extreme. In some species, such as acer or black locust, the living wood tibers are formed during the later period of a growing season. Their protoplast remains after the development of a cell wall and stores many starch grains in the cytoplasm for several years. Therefore, the mature xylem i n the sapwood is composed of ray and axial parenchymacells and sometimes the living wood fibers as the cells have aprotoplast.The
Formation Ultrastructure and
of Cell Wall
33
8 5
.. B
l I
FIGURE 28 Light (a) and electron (b) micrographs of transverse sections of S? depositing tracheids from Cryptomeria japonica. Areas of some cell organelles, for instance, Golgi bodies (Go), were measured with electron micrographs such as those shown in (b).
Fujita and Harada
9
B
r 6 S 4
3 2 1
0
0
c e l l number
C
RE
SI
s?r
Sam
Sar
S3
F
FIGURE 29 Changes of cytoplasmic volume during the differentiation of normal wood tracheids and proportions of some cell organelles at the stages of RE, S , , early S2, middle S,, late S?, S,, and F in Cryptonzeriu jqoniccr (see Figs. 28a and 28b).
FIGURE 30 A change of cytoplasmic volume during the differentiation of compression wood (see Fig. 28a).
Formation Ultrastructure and
Wall
of Cell
35
cytoplasmic features of these living cells are affected by the season, and also some of them seem to be specialized in their cell shape and cytoplasm. That is, the cells surrounding a vessel, particularly those directly contacted, become envelope-shaped and are very rich in Golgi bodies, r- and S-ERs, ribosomes, and mitochondria common to cells of active phase. On the other hand, their storage function seems to decay. These vessel-associated parenchyma cells are shown to concern the transportation of materials with vessel lumens [52,53] and also the formation of tyloses or gum that plugs the vessel lumen [55-571.
IV.
FORMATION OF WOOD CELL WALL
There is no doubt that cell walls are formed by the actions of cell organelles contained in each cell, even though some precursors of wall materials such as sugars may be supplied by the intercellular transport system.Therefore, cell wallformation is realized by the careful observation of cytoplasm that is undergoing cell wall development. It is also very important to select proper plant materials for precise examination of cell wall formation, becausegeneral plant cellsbearmanyphysiologicalfunctions in addition to cell wall formation. Moreover, the cell wall is composed of several types of chemical materials that are supposed to be metabolized by different cell actions, and their deposition on the wall may overlap. These complicated factorsare the major reason that the formation mechanism of plant cell walls has not yet been explained clearly, in spite of many investigations. Differentiating wood cells such as tracheids are very useful materials from this point of view. That is, they construct a very thick secondary wall, of which the ultrastructure and chemical components have been examined in detail, and the general sequence of cell wall formation can be traced through the series of differentiating cells along a radial row. Besides, the cell organellespossessed by thesecells are concernedonlywith cell wall formation, except vacuolation for the turgor pressure. In addition, if the depositing phase of individual wall materials such as cellulose, lignin, or hemicelluloses can be detected separately in differentiation, the relationship of cell organelleswith the metabolism of those materials would be grasped more clearly.
A.
CelluloseMicrofibrilDeposition
Cellulose is the mostbasic cell wall material in thewhole plant and it constructsthe framework structure of cell walls in the form of crystalline microfibrils as mentioned in Section 11. The formation has been studied using various plant cells from lower plants such as fungi or algae, to higher plants. Plasma membranes located just inside developing cell walls seem to be the most important cell organelles in relation to cellulose microfibril deposition. Although cross-sectional structures composed of unit membraneshadbeen observed by ordinary electron microscopic methods such as chemical fixation and ultrathin sectioning, faceviewsalongthemembranebecamepossiblewith the development of freeze-fracture or etching methods coupled with replication. Small particles on the outer surface of plasma membranes had been reported in various plant cells. The epoch-making discovery, however, was the characteristic assembly of granules located in the interior of the plasma membrane and revealed on the fractured surface in green algae such as Oocystis, Myclusteriu, or Vcloniu [58-601. Interesting structures have been reported using mainly single or naked cells such as algae [62], actobacteria [63,64], and cotton fiber [61], which can be frozen rapidly.
Harada36
and
Fujita
Small granule assemblies at the tips of microfibrils are called the terminal complex. These granules are considered to be the enzyme for the polymerization of cellulose molecules and their alignment i n the conlplex in relation to crystallization [64]. In underevolvcd algae such as vrtlonicr, the assemblies are large and linear, corresponding to their thick microfibrils [62]. On the other hand, evolved plants have small groups called rosettes [6 11. Thus, the form of the complex is considered to be related to the shape of the cellulose microfibrils and also to the evolution of plants. The polymerization and crystallization of cellulose microfibrils have been surveyed in detail using AcetoDactor- . x - y l i t z ~ ( ~which ~/, produces a thin cellulosic thread [6S] and has various mutants (661. The sequence of cellulose synthesis described above has not been traced in differentiating wood cells yet, because the freeze-fracture method is difficult to apply to them. However, cellulosic frameworks of wood cell walls are supposed to be constructed by a similar way. perhaps by a rosette. Although the freeze-fracture method isvery effective for visualizing characteristic structures such as the terminal complex on the membrane, the overall structure of differentiating wood cells depositing cellulose microfibrils must be examined by ordinary sectioning methods. Especially in wood cells depositing secondary wall layers, a control lnechanism for microfibrillar orientation is a very interesting viewpoint. Also, as the cellulose deposition is accompanied by the synthesis and accumulation of hernicclluloses and lignin, actions of various cell organelles must be traced in detail. Hence, the deposition phase of cellulose microfibrils i n differentiating tracheids can be traced in both normal and reaction woods. The phase can be detected by the increment of cell wall thickness (671, by means of autoradiography [68-70] (Fig. 3 l ) , and by chemical analysis of selectively collected rnaterials in some developing stagesof tracheids [ 7 I 731 and wood fibers [74](Fig. 32). The results obtained by these methodsshow that cellulose microtibrils are supplied to the wall mainly in the early and middle phases of the S, and S2 deposition stages. In addition to these deposition stages of cellulose microfibrils, most noticeable were the deposition of the G layer in the tension wood fibers and the S, thickening stage in the compression wood tracheids. This stage is composed of the deposition of cellulose microfibrils and is followed by the depositing stages of hemicelluloses and lignin. Compared with other differentiating stages of tracheids and wood fibers, the cytoplasm of cells forming the G layer isvery poor in its activity due to the fact that the region between the plasma membrane and the tonoplast is very narrow and cell organclles are rare there (Fig. 3%) 1751. The exceptionally abundant cell organelle in the cytoplasm is microtubules (MT). They are regularly distributed just inside the plasmamembrane (Pm), keeping a constant space of approximately 8 nm to the inner membrane and also between themselves (Figs. 33a and 33b). They are exactly oriented parallel to the depositing cellulose microfibrils in the stages of the G layer as well as the S , and S2 layers (Fig. 33b). The diameter of the microtubules is approximately 23 nm, and their numbers increase up to 20 per I p m of the plasma membrane, as calculated by their transverse direction. This abundant distribution results in the covering of about 40% of the cytoplasmic surface (Fig. 33b). A feasible link between the microtubules and the inner layer of plasma membrane is also discernible (Fig. 3321).These characteristics strongly suggest that microtubules and plasma membrane comprise the outermost complex of cytoplasm. On the other hand, there are only traces of Golgi bodies, S- and r-ERs, and the vesicles derived from them in the cytoplasm, in spite of the very active synthesis of cellulose microfibrils in this phase of the cell. On the contrary, in the beginning of the S, thickening stage of compression wood tracheids, in which cellulose microfibrils are supplied to the wall at 45" to the cell axis,
Formation Ultrastructure and
of Cell Wall
37
FIGURE 31 Serial light microscopic autoradiographs of “before section treatment” (a) and “after sectiontreatments”(b)withsodiumchloriteandhot 1.3% H,SO, from the differentiating compression wood tracheids in Cryptomeria japonica administered with 3H-glucose. Silver grains in (b) show the specific incorporation of radioactivity only on the inner surface of S , and S2 thickening tracheids, which reflects the deposition of cellulose by way of “apposition.” Removed activity can be detected in the intercellular layer of cells in the S , stage (arrows) and in the preexisting secondary wall of cells in the late S2stage (cells marked by an asterisk)by a comparison between (a) and (b) that implies lignin and hemicelluloses are supplied to the wall by wall of “intussusception.”
Harada38
and
Fujita
FIGURE32 Electron microscopic autoradiographs showing the incorporation of ‘H-phenylalanine in the transitional cell from S , to Sz,namely, in the stage of I-lignification (a), and from S , to S, in the stage of S-lignification in Cryptomeria japonica. Radioactivity can be observed around the intercellular layer and also within the Golgi bodies and vesicles in (a). In (b), vesicular inclusion is supplied to the wall by exocytosis (arrows) and radioactivity is often detected in such vesicles and the secondary wall.
cytoplasm isvery dense andwide. A similar complex between the microtubules and plasma membrane, however, is still observed [76]; microtubules are very abundant beneath the plasma membrane, having a link to it (Fig. 34a). The direction of microtubules is also in this case parallel with depositing cellulose microfibrils. Various cell organelles in the cytoplasm, such as Golgi bodies or ER, were shown to be involved in the synthesisof lignin precursors for the succeeding lignin deposition into the S, layer (see the next section). The characteristic appearance of microtubules is always applied to the cells depositing other wall layers such as S , , S2,and S3 without exception. It is interesting to note that the reorientation of microtubules precedes that of depositing cellulose microfibrils in the transition from the completion of a wall layer to the initiation of the next layer (Fig. 35). Moreover, the treatment of colchicine in which microtubule construction is obstructed by the formation of conjugation with microtubule protein “tubulin” resulted in a remarkable disturbance of depositing cellulose microfibrils (Fig. 36) [77,78]. These results clearly show that although microtubules present inside the plasma membrane cannot readily synthesize long and rigid microfibrils, these are involved in a great extent in the control of depositing cellulose microfibril orientation.
Formation Ultrastructure and
of Cell Wall
39
FIGURE 32 Continued
B. LigninDeposition Lignin is a very important cell wall component, particularly in wood cells, for the enhancement of the physical properties of cell walls and also for sealing the wall from prevention of waterleaks.Fortunately,lignincan be detected under an ordinary light microscope with the use of several stains such as a Wiesner reagent and Maule color reaction. Ultraviolet microscopy is especially useful for the quantitative analysis of lignin distribution in the cell wall [79] and more useful for studying the types of lignins present in the cell wall [80,81]. Needless to say, transmission electron microscopy coupled with potassium permanganate staining [82] or hydrofluoric acid treatment [83], electron probe microanalysis [84], and autoradiography [85-901 are also very useful for the observation of lignin from various points of view. The lignification of tracheid walls is generally known to last for a long period, from the S, stage to theF stage [79]. During this period, the lignification starts at the cell comer, spreads into the intercellular layer, and extends centripetally to the secondarywall. Lignin deposition, however, should be examined more closely in relation to the deposition of cellulose and hemicelluloses on each wall layer. This was attempted in the differentiating tracheids of compression wood, which were convenient for separating thelignification of the I region and S region because of their conspicuously highly lignified secondary wall, especiallyattheouterregion of the S, layer [67]. It has been shownthatthelignin deposition can be separated into two lignification stages, namely, I- and S-lignification. The former is active only during the early stage of secondary wall thickening, mainly at
40
Fujita and Harada
FIGURE 33 Electron micrographs of the cytoplasm-cell wall region of a transverse section from a tension wood fiber of Populus euramericana depositmg G layer (a) and of an obliquely sliced section from a S,-depositing fiber (b).
the S , stage, and is soon finished. The shape of I-lignification seems to stop the enlargement of cell size and adheres firmly between neighboring cells. On the other hand, the latter proceeds mainly after the development of a secondary wall framework, even though it begins at the middle phase of S , thickening. At any rate, lignin precursors permeate deeply into the cellulose microfibril framework of both primary and secondary walls and accumulate by way of “intussusception.” These two types of lignification were also applied in the differentiationof normal wood tracheids[86,91,92]. Moreover, when the speed
Formation Ultrastructure and .
.
Wall
of Cell
41
..... .,v*
(b) FIGURE 33 Continued
of lignin accumulation and the distribution of peroxidase were compared between the two regions [86], I-lignin seemed to be richer in the “condensed-type lignin” caused by the bulk polymerization than the S-lignin. This would be so because lignification proceeds with the higher content of lignin monomers and peroxidasein a rather large space without microfibrils. This assumption was confirmed by selectively labeled precursors coupled with light microscopic autoradiography [89,90]. When the lignifying cells are observed from the viewpoint of cytology, the cytoplasm is wider and denser than that of cells depositing cellulose microfibrils. Especially in the compression wood tracheids, an enormous amountof lignin precursors must be synthesized
Harada42
and
Fujita
Q t
p
FIGURE 34 Electron micrographs of 45"-inclined sections from compression wood tracheids in Cryptomeria japonica. (a) Shows the cytoplasmic feature in the cell just beginning S , deposition. At the cytoplasm-cell wall region (enlarged view), the distribution of microtubules (MT) is similar to that in Fig. 33a, although the cytoplasm is full of cell organelles, especially Golgi bodies. (b)
Shows the huge ridges and cavities in the of Golgi vesicles.
S , layer and poor cytoplasm after the active exmytocis
in their cytoplasm and thentransported from the cytoplasm to the wall. The area of cytoplasm becomes wider at the S , stage and also at the transition from Szto F (Fig. 30), where the cytoplasm becomes rich in Golgi bodies (Go) and ER (Fig. 34a). Although small vesicles (v) are produced mainly from Golgi bodies, they do not move to the cytoplasmic surfaceyet. These small vesicles increasein number and grow larger, occupying
43
Ultrastructure and Formation of Cell Wall
I
FIGURE 34 Continued
the largest part of the cytoplasm during the following late phase of the S, stage. S-lignification at the F stage is characterized by the active fusion of the well-developed vesicles to the plasma membrane and by the release of the vesicle inclusion to the wall area, namely, exocytocis. The cytoplasmic area resultsin the formationof an empty region after lignification (Fig. 34b). This sequence indicates thatlignin precursors are synthesized and stored in the vesicles that havebeen derived from Golgi bodies and on occasion from ER. In fact, the process was proven by autoradiography using tritiated lignin precursors [ S S ] . These sequences were also examined inboth lignifications at the I and S regions of normal woodtracheids(Figs. 32aand32b) [86]. InS-lignification, S-ER seems to be related to the lignification in addition to the Golgi bodies (Fig. 29), whereas I-lignification
Harada44
and
Fujita
;S1
FIGURE 35 Electron micrograph of an obliquely sliced cytoplasm-cell wall region from a tension wood fiber of Populus euramericana, which is just traveling from S2to the G layer. Many microtubules (MT) are oriented parallel to the fiber axis, although several (large arrowheads) are still oblique. Fine striations in the cell wall (small arrowheads) show the deposition of the S layer, and cellulose microfibrils of the G layer cannot be detected yet.
is performed mainly by the action of Golgi vesicles, similar to the case of compression wood tracheids. The lignin of compression wood tracheids is generally known to be rich in the condensed-type lignin. The cytoplasmic features of these lignifying cells seem to be consistent with the types of lignin suggested by Takabe et al. [86]. That is, the I- and S-lignins of compression woods and also the I-lignin of normal wood are metabolized mainly by Golgi bodies and the derivative vesicles, being richin the condensed-type lignin,
Formation Ultrastructure and
of Cell Wall
45
FIGURE 36 Scanningelectronmicrographs of theinnersurface of the developing S, layer of Crytomeria compression wood tracheids after incubatlon withoutcolchicine (a) and with colchicine (b). (a) Shows remarkably developed ridges and regularly depositing cellulose microfibrils parallel with the ridges, whereas (b) shows the disturbed deposition of them.
whereas the S-lignin of normal wood is synthesized through the cooperation of Golgi bodies, S-ER, and their vesicles, resulting in noncondensed-type lignin. It is interesting to note that the cytoplasmic regions becomewider, corresponding to both lignifications in the I- and S-regions in both normal and compression woods (Figs. 29 and 30). In addition, the peak of the S-lignification of compression wood is bigger than that of normal wood. The tendency of these peaks is to respond to the absolute amount of lignin that will be supplied to the separate wall regions. The precursors of lignin are most likely synthesized in the cytoplasm and stored temporarily, and then released from the cytoplasm to the wall, whereas the cytoplasm may possibly be rather narrow during the active depositing phase of cellulose microfibrils.
C.
HemicelluloseDeposition
Examination of hemicellulose deposition is divided into two groups. One covers the microscopic observations [68-70,931; the other is the chemical analyses of the tissues or cell walls collected selectively [71-741. Although the use of microscopy is a prerequisite for the observation of the microlevel localization of hemicelluloses, the specific staining method has not been improved enough to be applied on each hemicellulose and even mixed ones, being difficult to distinguish from cellulose or lignin. If any specific radio-
Harada46
and
Fujita
active precursor of each hemicellulose can be applied to the differentiating xylem, autoradiography will provide invaluable information on the deposition of hemicelluloses. A similar effect, although applied only to the total hemicelluloses, was achieved by a combined technique involving autoradiography and the removal of hemicelluloses from the tissue [93] or sections [53] that had been administered with tritiated glucose as the general source of cell wall materials. It becomesclear by these methods that hemicelluloses, although not so deeply as in the cases of lignin, accumulate in the preexisting framework of cellulose microfibrils by way of “intussusception” (Fig. 31). The depositing phase also intermediates the deposition of cellulose microfibrils with lignin accumulation. The deposition of each hemicellulose must be traced by the sugar analyses of tracheids or wood fibers selectively collected from the differentiating zone according to their development. This technique was achieved qualitatively by Meier et al. [7 l ] and improved quantitatively by Takabe et al. [73]. Judging from the content of polysaccharides in wood cell walls and the sugar constituents of hemicelluloses, glucose, mannose, xylose, arabinose, and galactose are, respectively, reflected in cellulose, glucomannan, arabino-gluconoxylan, and galactoglucomannan. As shown in Fig. 37a, mannose is supplied to the wall just after the cellulose microfibril deposition, followed by the deposition of xylose in the tracheid differentiation. In the case of wood fibers (Fig. 37b), xylose deposition follows directly the deposition of cellulose microfibrils. On the contrary, galactose and arabinose seemto be supplied to the walltogether in both stages of I- and S-lignification. The disagreement between the depositing manners of xylose and arabinose, namely, arabinose showing more affinity for lignin than xylose, may suggest that a chain of arabino-glucurono-xylan is not polymerized at one time but separately. That is, in concert with lignification, arabinose may be added, possibly as a side chain of the backbone of xylan already deposited.
I 0’
1
.
.
.
.
.
.
.
.
a
’
.
L
1 2 3 4 5 6 7 8 9 1 0 1 1 1 2 f rdctlonnumber
i r d c t l o nn u m b e r
Glucose
4 2 - 9
Hannole-A-,
rylor~-A-r
Ardblnose
- 0 - 1
GdIdctore”.--.
FIGURE 37 Depositionofpolysaccharidestocell wall duringdifferentiation ofnormalwood tracheids in Cryptomeria japonica (a) and of normal wood fibers in Juglans sieboldicrna (b).
Ultrastructure and Formation of Cell Wall
47
According to this speculation, galactose is also supplied to the glucomannose chain. On the other hand, chemical analyses of wood offer the evidence that groups of galactose, arabinose, and 4-0-methylglucuronic acid are combined directly between the polysaccharide and lignin in the so-called lignin-carbohydrate complex [941. These lines of evidence strongly suggest that the sugar groups forming branches of hemicelluloses are the ignition site of lignin accumulation. When the depositing periods and types of cell wall materials are coordinated with one another, the wood cell wall is concluded to develop by the following four processes: the appositional deposition of cellulose microfibrils on the preexisting wall, resulting in the construction of a framework of cell walls; the supply of hemicellulose main chains around the cellulose microfibrils and the reinforcement of the framework; the addition of hemicellulose branching chains such as galactose or arabinose;lignin accumulation starting on the branch and encrusting almost all spaces between the framework. The cytoplasmic relation to hemicellulose deposition has remained uncertain at many points. However, in contrast to the case of cellulose microfibrils that are synthesized at the surface of cytoplasm, the precursors of hemicelluloses are surely metabolized in the cytoplasm, judging from the combined observations from autoradiography and chemical treatments 1691.
REFERENCES D. A.Kribs. Bot. Gn:.. Y4:547 (193.5). H. A. Core, W.A. C M . and A. C. Day, Wood Structure r r t d Idmtijiccrtiorz. 2nd ed.. Syracuse Univ. Press. New York, p. 30 ( I 979). 3. J. F. Revol and D. A. 1. Goring. Wood Sei.. 14: 120 (1982). 4. J. Sugiyama. H. Chanzy, and J. F. Revol. Plmtcr, /Y3:260 (1994). S . H. Yamamoto and F. Horii. M~rcronlolrcrrlc.~, 26: 13 13( 1993). 6. J. Sugiyama, R. Vuong. and H. Chanzy. Mrrcror?loleclt/c.s,24:4168 ( 1991). I. 2.
7. A. Frey-Wyssling. Scirrm,, //Y:80 (1954). 8. A. hey-Wyssling and K. Muhlethalcr. Mrrkrortlol. Clwrn., 62:25 (1963). 9. R. D. Preston and J. Cronshaw. Nature, 18/:248 (1958). I O . K. Miihlethaler. Bioh. Z. S c h ~ ~ i :For.stwreitf.. . 30:55 (1960). I I . K. Miihlethnler. i n Ccllltlrrr Ultrtrstrrrcturc~of Wooc!\ Plat1t.s (W.A. C W . Jr., ed.).Syracuse Univ.Press,NewYork. p. 191 ( 1965). 12. V. Bnlnshov and R . D. Preston, Ncrtrrw. 176:64 ( 1955). 13. H. Haradn and T. Goto, i n Ce//lrlo.sc, t r t d Other Ntrt/trrr/ PnlynrcJr .Sy.stcr/r.s (R. M. Brown. Jr.. ed.). Plenum Publishing, New York. p. 383 (1982). 14. A. N. J. Heyn. J . Cell Biol.. 2Y: I81 (1966). I S . J. Sugiyama. H. Haroda. Y. Fujiyoshi. and N. Uyeda. Pltrr~ttr.Ihh: I61 ( 1985). 16. J. Sugiyomn. H. Harada. Y. Fujiyoshi. and N. Uycdo. Moku:tri Gtrkktrishi. 31:6 I ( 1985). 17. J. F. Revol. J . Mrrtrt: Sci. Lett.. 4 : 1347 ( 1985). 18. K. Muhlethaler. J. P o / w w r Sci.. C2N:305 (1969). 19. A. J . Kcrr ancl D. A. I. Goring. Wood Sci.. Y: I36 ( 1977). 20. K.Rue1 and F. Barnoud, ISWPC Stockholm. I : I I (1981). 31. Y. Kataoka. S. Saiki. and M. Fujita. Mokrr:rri Gnkkctishi, 38:327 (1992). 32. T. Kerr and 1. W. Bailey. ./. A r d d Arborotrr/r~,/5:327 ( 1934). 33. P. A. Roelotken. i n A d 1 w r x ~ c . sirr Bo/trrlictr/ Rc,srtrrch. Vol. 2 (R. D. Preston. d . ) . Academic Prcss. L,ondon a n c l NcwYork. p. 69 ( 1959). 24. A. B. W d r o p . A r ~ s t r d ..I. Hot.. h:299 ( 1958). 25. J. C. Rolnnd, B. Vam. and D. Reis. J . Cc,// Sci.. / Y : 1 3 9 (1975). 36. T. Fujii.Pl1.D.thesis.KyotoUniversity.Kyoto. Japan. 1981.
48
Fujita and Harada
27. 28. 29. 30. 31. 32.
H.Saiki. Mokuzui Gcrkkniski. /6:237 (1970). A.B.Wardrop. Hol;forschurlg, //:l02 (1964). Y. Imatnura,H.Harada,andH.Saiki, Bull. Kyoto Univ. For(>st,s,44: I83 ( 1972). H.Harada. Y. Miyazaki,andT.Wakashima, Bull. Go~vr.Forest Exp. Stu., 104:I ( 1958). K.Yamanaka,M.S.thesis,KyotoUniversity,Kyoto.Japan. 1969. R. D.Preston, The. Physictrl Biology of’ PlLmt Cell Walls. Chapman & Hall,London.p. 302
33. 34. 35. 36. 37. 38. 39. 40. 41. 42. 43. 44. 45. 46. 47. 48. 49.
SO. 5 1. 52.
53. 54. SS.
56. 57.
58. 59. 60. 61. 62.
63. 64.
65.
( 1 974). J . C.RolandandM.Mosiniak, IAWA BM//.,4:15 (1983). K. Kobayashiand N. Utsumi,unpublishedresults, 1951. N.Mori.M.Fjita,H.Saiki,andH.Harada, Bull. Kyoto U n i ~Forc..st.s,55:299 (1983). J. Cronshaw. Protoplasnl, 60:233 (1965). K.Takiya.H.Harada, and H. Saiki, Bull. Kyoto U I I ~ IForests, ! 48: 187 (1976). J. Ohtani, Bull. College Exp. Forests Hokkaido u/1j\J.. 33:4()7 (1979). R . A.Parhamand W. M.Baird, Wood Sei. Techrd., & l (1974). K.Kishi,H.Harada.andH.Saiki, Bull. Kyoto Unit,. Forc..sr,s.4Y:122 (1977). K.Kishi,H.Harada,andH.Saiki. Mok~cztriGtrkkaishi. 25521 (1979). S. Fujikawaand S. Ishida, Mokuzni Gakknishi, 2/:445 (1975). S. C. Chafeand G. Chauret, Protoplasm. ;YO:129 (1974). T. Fujii.H.Harada.andH.Saiki, Mok~rzniG~lkk
.st.s, IJ. SO: 183 (1978). M.Fujita. Y. Shoji, and H. Harada, H u l l . Kyoto Urli1: Forrsts, 4Y: I16 (1977). N. Shibata,M.Fujita,H.Saiki.andH.Harada. &dl. Kyoto U I I ~ Forc..sts. IJ. SO: 174 (1978). R. M.Brown.Jr..and D. Montezinos, Proc. N d . Accrd Sci. USA. 73: l43 (1976). T.ltohand R. M.Brown,Jr.. Plarrtcr. /60:372 (1984). D.Montezinos,in The Cytoskeletou i r ~Plrrrlt Gron,th ctrld 1 l e w l o p r ) w ~ t(C. W. Lloid, ed.). Academic Press, London, p. 147 (1982). J. H. N. Willison, J. Appl. Po1yr11c.rSyrnp., 3791 (1983). A.M. C. Emons, i n Bio.syntlw.sis m r l BiotlrRrcr~lrtiorl (fCellulo.se (C. H.HaiglcrandP. J. Weimer, eds.). Marcel Dekker, New York. p. 7 I ( 1991). K. Zanr, .l. Cell Rio/.. A0773(1979). C. H.HaiglerandM.Benziman,in Cellrrlow C ~ I Other I ~ NLrturrrl Polyrr~crSy.sterr~.s(R. M. Brown, Jr.. ed.). Plenum Press, p. 273 (1982). C. H. Haigler, in Bio.syrrt/w.si.s c r r d Hioclrgrcrdrrtiorl o f Cdlulosc~(C. H. Haigler and P. J. Weimer,
eds.). Marcel Dekker, New York, p. 99 ( 1991). 66. S. Kt~ga,S. Takagi.and R. M.Brown, Jr., Polyrr~er.343291 (1993). 67. M.Fujita,H.Saiki,andH.Harada, Moklrzai Gakktrishi, 24:158 (1978). 68. M.Fujitaand H. Harada. Mokuzcri Gnkkaishi,24:435 (1978). 69. M.Fujita. K. Takabe.andH.Harada. Mokuzri Gdkoixhi. 27337 (1981). 70. K.Takabe.M.Fujita,H.Harada,andH.Saiki. Mokuzcri Gokknishi. -?(l:103 (1984). C. B.Wilkie. Hol~fi)rsckurlg,13: l77 (1959). 7 1. H.MeierandK. 72. H.Meier,in Bio.syr~rhe.si.sc m 1 BioLI~.grcr~Irriorlof’ Wood Corr~porz~r~ts (T. Higuchi. ed.). Academic Press. New York
(1985).
Ultrastructureand Formation of Cell Wall
73. 74. 7s. 76. 77. 78. 79. 80. 81. 82. 83.
84. 85. 86. 87. 88.
89. 90. 91. 92. 93. 94.
49
K. Takabe, M. Fujita, H. Harada. and H. Saiki. Mok~czoi GNkkaishi, 29:183 (1983). K. Takabe, M. Fujita, K. Tanaka, and H. Harada, Bull. Kyoto CJniv. Forests. .56:234 ( 1984). M. Fujita, H. Saiki, and H. Harada, Mokuzui Gakkaishi,20:147 (1974).
M. Fujita, H. Saiki, and H. Harada, Moktczai Gnkkaishi, 24:355 (1978). J. D. Pickett-Heaps, D e ~ dBiol.. /5:206 ( 1967). M.FijitaandH.Harada.“Colchicinetreatmentandmicrolibrilorientationindifferentiating compression wood tracheids,” Proc.. 27th A n r l d Meetirrg of Jup,crrwsc~Wood Resectr-chSociety. p. 311 (1977). A. B. Wardrop, TAPPI, 40:22S (l9S7). B. J . Fcrgus and D. A. I . Goring, H o l ~ f o r . s c l ~ ~ c24: r ~ 118 g , (1970). A. Yoshinaga, M. Fujita, and S. Saiki, Mokuzcli Gnkknishi, 38:629 (1992). M. Mauer and D. Fengel, Hol;for.schurlg. 44:4S3 (1990). I . H. Clark, TAPPI, 45:310 (1962). S. Sakaand D. A. I. Gorgin.in Biosy1lthesi.s crrltl Riorlesmrltrtiorl of’ Wood Cort~pot~c,r~t.s (T. Higuchi. ed.), Academic Press, New York, p. S 1 (1983. M. Fujita and H. Harada, Mokuzai Gakknishi, 25:89 (1979). K. Takabe, M. Fujita. and H. Harada. Mokuzcti Gtrkknishi, 31:613 (1985). N. Terashima. K. Fukushima, and K. Takabe, Holifi)r.sc~hwzg,40(Suppl.): 101 ( 1986). K. Fukushima and N. Terashima, J . Wood Cllern. T e c h o l . , /0:413 (1990). N. Terashima and K. Fukushima. Wood Sci. fi~cl~nol., 22:2S9 (1988). K. Fukushima and N. Terashima, Hol;fi~rsc.hur~g. 45:87 (1991). M. Fujita, K. Takabe, and H. Harada, ISWPC (Tsukuba), !:l4 (1983). K. Takabe, M. Fujita, H. Harada, and H. Saiki, Mokuzai Gczkkaishi, 27:813 (1981). P. M. Ray, J . Cell Biol.. 3.5:660 ( 1967). D. Fengel and G. Wegener, Wood, Walter de Gruyter. Berlin, 1984.
This Page Intentionally Left Blank
Chemical Composition and Distribution Shiro Saka Kyoto University, Kyoto, Japan
1.
INTRODUCTION
Wood is a complex of natural polymer substances: cellulose, hemicelluloses, and lignin. These polymer substances are not uniformly distributed within the wood cell walland their concentrations change from one morphological region to another. In order to understand the physical and chemical properties of wood, it is essential to study the topochemistry of these polymer substances. This chapter, therefore, deals with chemical composition andits distribution in normal and reaction woodsfrombothsoftwoodandhardwood species.
II. GENERAL FEATURES OF WOOD CELLS Woody plants have several different types of cells in bothsoftwoodsandhardwoods. However, the anatomy of softwoods is less complex than that of hardwoods. In softwoods, the principal types of cells are tracheid and parenchyma, whereas those in hardwoods are fiber, vessel, and parenchyma.Sincesoftwood tracheids andhardwood fibers constitute the majority of wood cells, they contribute in a major way to the physical and chemical properties of wood. The cell wall organization of typical softwood tracheids or hardwood fibers [ 1,2] is described in Fig. 1 . Basically, the cell wall consists of the primary (P) and secondary (S) wall layers. The P layer is formed during the surface growth of the cell wall, and the S layer is formed during the thickening of the cell wall. This layer is composed of three sublayers termed S , , Sz, and S3, based on differences in microfibril orientation. A layer called middle lamella (ML) is located between adjacent cells. Since it is difficult to differentiate the ML from the two P walls on either side, the term compound middle lamella (CML). which encompasses the ML and the two adjacent P wall layers, is frequently used (Fig. 2a). The pattern of the cell wall organization in reaction wood is somewhat different from that of normal wood [31. Compression wood, developed on the lower side of a leaning softwood stem or branch, lacks the S, layer but contains an extra layer of lignin [%(L)] located between the S , and S, layers (Fig. 2b). Tension wood, formed on the upper side of a leaning hardwood stem or branch, often lacks one or more of the three secondary 51
52
Saka
FIGURE 1 The gross structure of a typical softwood tracheid or hardwoodfiber.(Courtesy Prof. Emer. R. J. Thomas, North Carolina State University, Raleigh, NC.)
of
wall layers. Instead, the gelatinous layer (G layer) is usually deposited adjacent to the cell lumen (Fig. 2c). The G layer contains little or no lignin and consists mainly of cellulose microfibrils oriented parallel to the fiber axis.
111.
CHEMICAL COMPOSITION OF WOOD
A.
Normal Wood and Reaction Wood
The chemical constituents of wood are well known,and a numberof authors have provided an excellent review of this work [4-81. The major cell wall constituents are cellulose, hemicelluloses, and lignin. Other polymeric constituents, present in lesser and often varying quantities, are starch, pectin, and ash for the extractive-free wood. Tables 1 and 2 show comparisons of the chemical composition made by Time11 [9] for five hardwoodsand five softwoods, respectively. Although the cellulosecontent is more or less the same (43 -t 2%) for both groups, the hardwoods contain less lignin. The lignin content of hardwoods is usually in the range of 18-25%, whereas that of softwoods varies between 25% and 35%. However, tropical hardwoods can exceed the lignin content of many softwoods. The structure of lignin is different between these two groups: softwood lignins are composed mostly of guaiacyl units, whereas hardwood lignins consist of syringyl and guaiacyl moieties [ 101. The hemicelluloses found in these groupsvary both in structure and quality, as shown in Fig. 3. The predominant hardwood hemicellulose is a partly acetylated, glucuronoxylan (O-acetyl-4-O-methylglucuronoxylan),accounting for 20-35%, whereas softwoods containglucuronoarabinoxylan (arabino-4-0-methylglucuronoxylan)in therange of 10%. Hardwoods contain only a small quantityof glucomannan. In softwoods, however, a partly acetylated galactoglucomannan (0-acetylgalactoglucomannan) makes up as much as 18%. In additiontothesemajorcellwall components, pecticmaterialsandstarch are included in much smaller quantities inboth softwoods and hardwoods. Ash usually makes up between 0.1% and 0.5% of wood, but tropical species often exceed this range. Wood
FIGURE 2 (a) Cross section of brominated normal wood tracheids in Douglas fir [Pseudotsuga rnenziesii (Mirb.) Franco]. Transmission electron micrograph of ultrathin section. Dark zones indi-
cate the higher lignin concentration. (b) Cross section of compression wood tracheids in eastern white pine (Pinus strobus L.). Ultraviolet micrograph of thin section (upper portion) shows high concentration of lignin in the S,(L) layer indicated by an arrow. Polarized light micrograph (lower portion) shows a lack of the S3 layer.
53
Saka
54
4 FIGURE 2 Continued. (c) Cross section of tension wood fibers in Enoki [Celtis sinensis Pers vat. japonica (Planch) Nakai]. Transmission electron micrograph of KMn0,-stained ultrathin section.
Note a nonstained G layer deposited following the stained Prof. Emer. H. Harada, Kyoto University, Kyoto, Japan.)
S2 and S3 layers. (Courtesy of the late
in heartwood also contains varying quantitiesof extractives that are always more abundant than sapwood. The chemical composition of reaction wood differs from that of normal wood. Table 3 shows a comparison made by Timell [ 1l ] of the average chemical composition of normal and compression woods of many conifers. Pronounced compression wood contains, on average, 39% lignin and 30% cellulose, compared to 30% and 42% for normal wood,
TABLE 1 Chemical Composition of Wood from Five Hardwoods"
Cell wall constituent Cellulose Lignin Glucuronoxylan Glucomannan Pectin, starch, ash, etc. "All values in percent of Source: Ref. 9.
Acer rubrum
Betula papyrifera
Fagus grandifolia
Populus tremuloides
Ulmus americana
45
42
45
48
51
24
19 35 3
22 26 3 4
21
24
25 4 2
24
extractive-free wood.
1
19 3 4
4 2
"
omposition Chemical TABLE 2
55
Chemical Composition of Wood from Five Softwoods"
constituent wallCell Cellulose 27 Lignin Glucuronoarabinoxylan Galactoglucomannan Pectin, starch, ash, etc.
A hies hulsarnen
42 41 29 9 18 2
Picea glauca
Pinus strobus
41
41 29 9 18
13 18 1
3
Tsuga canudensis
33 7 16 3
TI1uja occidentalis 41 31 14 12
2
"All values in percent of extractive-free wood. Source: Ref. 9.
respectively. The content of galactoglucomannan is only 9%, half that in normal wood. The amount of xylan, on the other hand,is the same in thetwotissues.Compression woodcontains 2% of a 1,3-linked glucanand 10% of a galactan,bothpresentinonly trace amounts in normal wood. With regard to chemical composition of tension wood, the most characteristic feature is that it contains less lignin andxylan described as pentosan, but has much more cellulose
Saka
56
TABLE 3 Average Chemical Composition of Normaland Compression Woods of Softwoods"
Cell wall constituent Lignin Cellulose Galactoglucomannan 1.3-Glucan Galactan Glucuronoarabinoxylan Other polysaccharides
Normal wood Compression wood
30
39
42
30 9 2 IO
18
Trace Trace 8 2
8
2
"All values in percent of extractive-free wood. Source: Ref. I 1.
and galactose residues than normal woods (Table 4) [ 121. Furthermore, higher ash and uronicacidcontentsarereportedfortension woodthanin the side woodof Japanese beech (Fugus crenuru Blume) [ 131. The higher cellulose content in tension wood is due to the presence of a gelatinous layer, which is often quite thick and unlignified (Fig. 2c).
B. Tracheids and Ray Cells The tracheids in softwood or fibers in hardwood constitute more than 80% of the cells found in wood; thus, the global analyses reflect moreor less the composition of these types of cells. However, the chemical composition of ray cells may not be inferred from that of the whole wood. The data in Table 5 reveal a comparison made by Hoffmann and Timell [ 141 between the ray cells and tracheids from red pine (Pinus resinosu Ait.). The defibrated samples after delignification by acid chlorite were subjected to the separation of tracheids and ray cells through screening, followed by subsequent analysis of sugar residues. As reported in the literature [ 151, the ray cells contain more lignin. somewhat less cellulose, only half as much galactoglucomannan, and the same amounts of xylan and pectin as do the tracheids. A small amount of a 1,3-linked glucan also present in the ray cells appears to be absent
Chemical Composition of NormalandTension Woods from Euccclyptus gonioc.rr1y.r"
TABLE 4
Cell wall wood Tension wood Normal constituent 13.8 Lignin 57.3 Cellulose Pentosan Acetyl 7.4 Galactose residue
29.5 44.0
1s. I
11.0
3.0 2.5
I .9
"All values in percent of extroctlve-free wood. Solrrcr: Ref. 12.
omposition Chemical
l
57
Normal wood
wood" Colnpresslon
Tracheids cells Ray Tracheids Ray cells Cell
(%)
(%)
(c/o)
(c/o)
Lignin Cellulose Galactoglucomannon 1,3-Glucan Tracc Galactan Glucuronoarabinoxylan Pectin Other polysaccharides
40
28 42 20 -
40 35 II 2
40 30
Trace
IO
10 I
7 I
I
1
35 9 2
Trace 11
2 I
8 1 1
9 2
"From Ref. 14. hFrom Ref. 18.
in the tracheids. Overall, the results in Table 5 are in good accord with those by Perilii [ 161 and Perilii and Heitto [ 171. However, these authors indicated more xylan in ray cells than normal tracheids i n Scots pine (Pirzus sylvesfris L.). The lower content of xylan in Table 5 is due possibly to partial removal during chlorite delignification. Also included in Table 5 are the chemical compositions of tracheids and ray cells from red pine compression wood [ 181. Although compression wood tracheids have a different chemicalcompositionfromnormalwood tracheids, the ray cells in compression wood are chemicallyindistinguishablefromthose in normalwood.Comparedwith the compression wood tracheids, the ray cells have the same contents of galactoglucomannan, 1,3-glucan, and xylan. However, the galactan typical of grosscompressionwood is missing.
C. Earlywood and Latewood Meier [ 191 has studied the effect of the cell wall thickness on polysaccharide content by comparing earlywood and latewood from normal Scots pine(Pirzus sylvesfris L.). As shown in Table 6, the latewood contains more glucomannan and less glucuronoarabinoxylan than the earlywood. Since the proportion of the latewood tracheid S I layer to the whole wood is greater than that of earlywood, the observed differences are due mainly to the thicker S2 layer in latewood tracheids. I t may therefore be concluded that the tracheid S I layer hasmoreglucomannanand less glucuronoarabinoxylanthan doothermorphological regions, which agrees reasonably well with the results of Whiting and Goring 1201 for the secondary wall and middle lamella fractions of black spruce (Picecr rnnriarzcr Mill.). Also shown in Table 6 are the results of compression wood balsam fir [Abies ~ N I sanlecr (L.) Mill] 1211. Although earlywood and latewood have the same content of lignin [22],thepolysaccharidecomposition is different betweenthesetwo tissues. It canbe speculated in a similar way that the tracheid S, layer in compression wood contains more celluloseandgalactoglucomannanbut less galactan,arabinan,andxylan that doother morphological regions of compression wood.
58
Saka
TABLE 6 Polysaccharide Composition of Earlywood and Latewood from Normal Scots Pine and Balsam Fir Compression Wood
Balsam fir compression wood’ Polysaccharide
pine”
Scots
Normal
Latewood Earlywood Latewood Earlywood (%l
Cellulose 56.2 Galactan 3.1 Glucomannan Arabinan Glucuronoarabinoxylan
(%)
(%)
56.7
45.0
3.4 20.3
19.0 16.0
50.4 15.0 18.7’
1.o 18.6
(%)
24.8 1.8
14.1
0.9
0.6
19.1
15.3
“From Ref. 19. hFronl Ref. 2 I . ‘Values as galactoglucomannan.
IV.
DISTRIBUTION OF POLYSACCHARIDES
A.
Introduction
The distribution of cellulose is probably the easiest to study at the various morphological regions of wood.Onepossiblemethodinvolves the useofholocellulose after desired poststaining with heavy metals such as uranyl acetate [23-2.51 and lead citrate [26]. Although the orientation of the cellulose microfibrils is quite different in the various cell wall layers, cellulose is quite evenlydistributedthroughout the secondary wall. In the primary wall, however, microfibrils are rather loosely and randomly arranged (Fig. l), so the concentration of cellulose in the primary wall may be lower than that of the secondary wall. Unlikecellulose, a study of the distribution of hemicellulose is difficult. This is because histochemical techniques are generally nonspecific and frequently unreliable. In order to overcome these difficulties, BouteljeandHollmark [27] introduced the use of interference microscopycombinedwithenzymatic treatment. Sinner et al. 128,291 used electron microscopy to study the enzymatic degradation of the cell wall components by xylanases, mannanase, and avicellase for delignified spruce [Picea abies (L.) Karst.] and beech ( F c q p s sylvaticcr L.). It was found that xylan concentration is rather high in the S , and S, layers for both woods. Hoffmann and Parameswaran [30] made another attempt to study the polysaccharide distribution in spruce tracheids through oxidation of polysaccharides with heavy metal. Subsequent electron microscopic observations indicatedthe highest concentration of hemicelluloses in the S , layer. Awano et al. [31] have recently applied immunoelectron microscopy to studying the distribution of glucuronoxylan in buna (Fagus crencrtu Blume). An extensive study in the future will provide useful information on its distribution. The distribution of polysaccharides also has been studied by examination of holocelluloseskeletonsafterremoval of lignin with acid chlorite [21],atechniquefurther refined by Fujii et al. 1321by using ultrathin sections. An electron micrograph of the holocellulose skeleton from the compression wood of tamarack [Lcrrix laricim (Du Roi) K. Kochj is shown in Fig. 4. Forcomparison, Fig. 5 shows a micrograph ofa lignin skeleton of thc same wood. Although the presence of the residual lignin and some removal
omposition Chemical
59
FIGURE 4 Holocellulose skeleton of two tracheids in compression wood of tamarack [Lark lurkina (Du Roi) K. Koch]. Note the low concentration of polysaccharides inthe S,(L) layerand absence of substances in the middle lamella region. Transmission electron micrograph of a cross section. (Courtesy of Prof. Emer. W. A. C M , Jr., State University of New York, Syracuse, W.)
of polysaccharides may obscure the data, overall the results obtained by this method are in good agreement with the holocellulose distribution inferred from the lignin skeleton seen in Figs. 4 and 5 [33]. Some other methods also have been proposed; Parameswaran and Liese [34] have given an excellent review of these studies. For the localization of pectin, Albersheim et al. [35] have used the hydroxylamineiron method developed by McCready et al. [36,37] for the quantitative measurement of pectin. With this method, Parameswaran and Liese [34] have found a homogeneous distribution of pectin across the secondary wall. The middle lamella also was found to be highest in concentration. The use of ruthenium red and alcian blue also is proposed for staining pectin substances [38-401. For quantitative determinationof the polysaccharide distribution, the microdissection technique has often been used. One of the oldest is Bailey’s work in 1936 [41] for the pentosan content determinationof the middle lamella in Douglas fir. In 1959, Meier [42,43] adopted a similar technique for hardwood fibers (Betula verrucosa Ehrh.) and softwood tracheids (Pinus sylvestris L. and Picea abies Karst.) at different stages of development
60
Saka
FIGURE 5 Lignin skeleton of threetracheidsin compression wood of tamarack [ L a r i x luricina (Du Roi) K. Koch]. Note the high concentration of lignin in the S,(L) layer as well as in the middle lamella region. Transmission electron micrograph of a cross section. (Courtesy of Prof. Emer. W. A. CBtC, Jr., State University of New York, Syracuse, NY.)
that were microscopically distinguished, isolated, and subsequently subjected to microanalysis for sugar residues. From a knowledge of the chemical composition of different polysaccharides in wood, the contentsof polysaccharides at various morphological regions could be calculated. Although some doubt exists as to additional deposition of polysaccharides during the later stage of the secondary wall thickening, the technique developed by Meier remains applicable [44]. Later, Norberg and Meier [45] isolated the gelatinous layer(G layer) in tension wood fibers (Fig. 2c)by using ultrasonic treatment. Subsequent analysisindicated that it contains 98.5% glucose and 1.4% xylose, suggesting thepure cellulosic nature of the G layer. Luce [46] determined the radial variationin the content of hemicelluloses in softwood tracheids by a chemical peelingtechnique.Burkeetal. [47] measured the sugar content of the polysaccharides in the primary walls of a suspension-cultured Douglas fir. In 1981, Hardell and Westermark [48] have developed a method for peeling layers of the cell wall from a slightly delignified single tracheid of Norway spruce [Picea abies (L.) Karst.]. They reported only small differences in the relative amounts of polysaccha-
omposition Chemical
61
rides between the compound middle lamella and the secondary wall, a finding that is not in agreement with Meier's results [42]. It appears that a treatment of slight delignification may cause a partial dissolution as well as redistribution of hemicelluloses. The arabinose and galactose contents for the compound middle lamella were foundto be 7.3% and 7.6%, values that are considerably lower than those from nonlignified wood [6]. More recently, Whitinget al. [49]developedanothermethod of preparing wood tissue fractions from the compound middle lamella and secondary wall of black spruce (Piceu nzariana Mill.) by taking advantage of the difference in density ( p ) between lignin ( p = 1.4 g/mL)andpolysaccharide ( p zz 1.5 g/mL).Themost significant finding after analyses of carbohydrates for these wood tissue fractions [20] was that the concentrations of celluloseandglucomannan are smaller in the middlelamellathan in the secondary wall, whereas the concentrations of other polysaccharides are more or less the same in both the secondary wall and the middle lamella regions. Compared to the previous methods by Meier [42] or Hardell and Westermark [48], the method of Whiting et al. [49] is more reliable, due to only the physical treatment of specimens without introducing any chemical changes.
B.
Distribution of Polysaccharides in Normal Wood
Whiting and Goring [20] conducted carbohydrate analyses of fractions of tissue from the middle lamella and secondary wall of black spruce tracheids. Figure 6 shows the relationships between polysaccharide content and lignin content for the various tissue fractions. Each fraction is amixtureof the secondary wall, primary wall, andmiddlelamella in varying proportions. The fraction with a lignin content of 22% is from the secondary wall tissue, whereas the extrapolated results to a composition at which the cellulose content becomes zero would represent the polysaccharide composition of the true middle lamella with a lignin content of 70%. Figure 6, therefore, shows that the middle lamella contains less cellulose and glucomannan but more galactan and arabinan than the secondary wall.
t
U
0.2
0.3
0.4
0.5
0.6
0.7
FIGURE 6 Polysaccharide content versus the lignin content for thevarious black spruce (Picecc tnnriat~nMill.). (From Ref. 20.)
tissue fractions of
Saka
62 TABLE 7
l481
Relative Polysaccharide Percentages of the Secondary Wall Tissue
Polysaccharide Cellulose Glucomannan Glucuronoarabinoxylan 12.8 Galactan
WhitingGoring and [201
Meier Hardell Westermark and [421 63.0
1.1
0.0
Arabinan
58.1
60.0
20.8
23.7
14.3
10.7
4.8 2.0
4.1 1.5
However, the concentration of glucuronoarabinoxylan is essentially the same in both morphological regions. For the secondary wall tissue, Table 7 shows a comparison made by Whiting and Goring [20] of the relative polysaccharide percentages measured by Meier [42] and Hardell and Westermark [48] on Norway spruce (Picea abies Karst.) and by Whiting and Goring [20] on black spruce (Picea nzariarza Mill.). The values of Meier were calculated using a proportion of 90% secondary wall and 10% middle lamella for the whole wood [50].It is apparent that the agreement between the results obtained by three investigators is good, particularly between the data by Hardell and Westermark and those by Whiting and Goring. It istherefore likely that in the tracheid secondary wall thecontents of hemicelluloses decrease in thefollowingorder:glucomannan,glucuronoarabinoxylan,galactan, and arabinan. A comparison of the relative polysaccharide percentages of the middle lamella-rich fractions is shown in Table 8 for the same three investigators. The results of Whiting and Goring are the composition at the 70% lignin content in Fig. 6, which would be representative of the true middle lamella. For comparison, data from tissue fraction with 39% lignin (Fig. 6) are also included. This fraction includes part of the secondary and primary wall tissues, as well as the middle lamella fraction. In contrast to the excellent agreement for the secondary wall fractions (Table 7), the results on the middle lamella are at variance with each other. This is because the middle lamella fraction is most difficult to prepare in a pure state. It should be noted that the cellulose content of 50.3% for Hardell and Westermark (Table 8) is not much different from the value of 58.1 in Table 7 for the secondary wall fraction. Additionally, the results by Hardell and Westermark are i n good agreement with the data from the tissue fraction of 39%)lignin content by Whiting and Goring. Thus,
TABLE 8
Relativc Polysaccharide Percentages of Middle Lamella-Rich Fractions Hardell and Westermark Meier ~421
Polysaccharidc
(-)
50.3 Ccllulose Glucomannan
33.4 7.9 13.0 16.4 29.3
13.3 Glucuronoarnbinox~lat~ Galactan Arnbinan
Whiting and Goring [20]
148I (4I % lignin)
(70%. lignin) 0.0
50.8
22.6
12.5
21.6
15.4
(39% lignin)
37.5 7.6 6.2
29.2 20.8
7.2 5.0
Composition Chemical
63
a sample collected by Hardell and Westermark must be to some extent contaminated with the secondary wall fractions. It is of interest to note that both the results of Meier for the compound middle lamella and of Whiting and Goring for the true middle lamella show glucomannan to be the lowest among hemicelluloses in the middle lamella region. For overall trendsof the carbohydrate distribution across the cell wall, Meier [42,43] has indicated that, although the cellulose content is very low in the ML (middle lamella) and P (primary wall) regions, arabinan is almost completely confined to M P regions, and galactan is almost completely confined to M P S , regions. Glucomannan, however, increases from M + P to the S , layer in softwoods and remains at a rather constant low level in hardwoods. Glucuronoxylan in hardwoods has a higher concentration in the secondary wall than in the M P. Figure 7 shows the distribution of polysaccharides across the woodcellwall of Cryptomeria tracheids obtained by Takabe [U] through the technique of Meier [42]. Interestingly, cellulose is rich in the middle of the S , layer, whereas hemicelluloses of glucuronoarabinoxylan and galactoglucomannan are abundant in the S , and outer parts of the S, and S3 layers. The warty layer (W) is composed mainly of galactoglucomannan.
+
+ +
+
C.
Distribution of Polysaccharides in ReactionWood
C6t6 et al. [21] also used the technique of Meier [42] to study the polysaccharide distribution in compression wood tracheids of balsam fir [Abies balsamea (L.)Mill.]. Figure 8 shows the results obtained. It should be noted that the glactoglucomannan, arabinan, and xylan are homogeneously distributed across the secondary wall, whereas a higher concentration of galactan was found in the outer regionof the secondary wall. This fact was later confirmed by Larson [5 1,521. The content of cellulose is, on the other hand, higher at the inner portion of the cell wall. For the compound middle lamella (P M P), the high
+
+
:.:.:.:.:* ....:.:\.:\..:.., >>: ....... .:.:.:.:.:................. ....... ,...... :., ... ..... .A.
............... .....:..
...
... ...
m Glucuronoarabrnoxylan 0 blactoglucomannan 0 tcllulorc
FIGURE 7 The distribution of polysaccharides across the wood cell wall of tracheids in Cryptomeria japonica D. Don. (From Ref. 44.)
64
Saka
Percent
GALACTAN
ARABINAN
CELLULOSE
ARAEINOGLUCURONOXYLAN
GALACTOGLUCOMANNAN
FIGURE 8 Graphical representation of the distribution of polysaccharides in compression wood tracheids of balsam fir. (From Ref. 21.)
content of arabinan and galactan would be due to high pectin content. It is reported that chemical composition of the primary wall is the same in normal and compression woods [5 1,521.
V.
DISTRIBUTIONOF LIGNIN
A.
Introduction
Unlike polysaccharides, a number of reliable methods can be used to study the distribution of lignin in wood. One of the oldest procedures is selective staining, followed by study under the light microscope[53]. Although some doubt exists as to this specificity for lignin [54,55], potassiumpermanganatestaining [56] has been usedextensivelyforstudying lignin distribution by electron microscopy [57-601. Also reported were studies by electron microscopy of lignin skeletons (Fig.5 ) created by the carbohydrate removal by brown-rot fungi [61] or concentrated hydrofluoric acid [32,62-641. Although some alteration of the lignin through condensation may result and the possible presence of residual carbohydrates may obscure the data, overall the results obtained by this method are in reasonable agreement with those from potassium permanganate staining [59]. Although the above methods are useful in elucidating the presence of lignin in the various morphological regions of wood, they can provide only qualitative evaluation of thelignindistributionacrossthecellwall. For quantitativevisualization of thelignin distribution, ultraviolet (UV) microscopy with thin sections of wood has provided good results. This method was initiated by Lange [65], who estimated the weightconcentration of lignin to be, respectively, 16% and 73% for the secondary wall and compound middle lamella of Norway spruce tracheids. This result was in excellent agreement with Bailey’s value of 71% for the Douglas fir middle lamella fractions obtained by a direct analytical method [66]. Previous to Bailey’s work, Ritter [67] had concluded that approximately75% of the lignin in wood is located in the middle lamella, with the other 25% being located in the secondary wall. Apparently, a distinct difference exists between the results by LangeBailey [65,66] and Ritter [67]. However, considerable confusion has appeared in the lit-
Composition Chemical
65
erature. Some of this confusion could be due to the use of the symbol o/o to denote both the percentage fraction of the total wood lignin contained in a particular morphological region and the lignin content of that region. Therefore, g/g. i.e., g of lignin/g of cell wall substance. is used in this chapter to denote lignin concentration. The symbol o/o is then reserved for the proportion of total lignin in a particular morphological region. Later. Goring and co-workers [68-701 refined the UV microscopy method through a preparation of the thin section (0.5 p m ) to avoid errors caused by nonparallel illumination. Goring et al. then determinedquantitatively the distribution of lignin in wood [50,70-751 and proved that the result by Lange-Bailey[65,66] was correct.They also proved that the conclusiondrawn by Berlyn and Mark [76] is correct. that the middle lamella region can contain at most 40% of the total lignin in wood due to its small volume fraction of wood. In addition to these, they discovered that different lignins occur in different types of cells and different cell wall regions of wood [72-741. More recently, through the use of UV microscopy, Yang and Goring [77.78] have found that the secondary wall lignin of softwoodscontains twice as many phenolic groupsas the middlelamella.This finding was later confirmed by Whiting and Goring [79] from a study of the secondary wall and middle lamella fractions. Of other methods for the quantitative assay of the lignin distribution, Lange and Kjaer [SO] proposed the use of interference microscopy, and Boutelje [811 later refined this technique.More recently, Saka et al. [82-861 developeda new techniqueforthe quantitative determination of the lignin distribution in wood. The method involves a specific bromination for lignin in a nonaqueous system (CHCI,). Bromine concentrations in the various morphological regions of wood are then determined by electron microscopy (TEM or SEM) coupled with energy-dispersive X-ray analysis (EDXA). By knowing the lignin reactivity toward bromination, the distribution of lignin can be determined for various morphological regions of wood. Figure 9 shows the direct comparison made between two techniques of UV microscopy and EDXA measurement in bromination [S61 over the
1 .oo Earlywood
Latewood
I
0
.-C .-
l
SECONDARY WALL
0
I
I
I
15
10
5
I
I
1
5
10
Cell number FIGURE 9 Variation of lignin concentrationsacrosstheearlywood/latewood boundary of black spruce measured by U V microscopy ( 0 ) and the EDXA technique ( 0 ) .(From Ref. 86.)
Saka
66
earlywood/latewood boundary of black spruce (Piceu r~zuriur~a Mill.). It is quite apparent that the agreement between the results obtained by the two methods is good. With this EDXA technique, another method has also been developed by Westennark et al. [87] and Eriksson et al. [SS], based on a mercurization of lignin, followed by determination of mercury concentration in different morphological regions of wood.
B.
Distribution of Lignin in Softwoods
Table 9 shows the distribution of lignin in tracheids of black spruce (Picea marianu Mill.) as determined by UV microscopy [50]. The results show that the lignin concentration in the secondary wall (S) is considerably lower than that in the middle lamella (ML or ML,,). However, the secondary wall makes up a muchlarger proportion of the total tissue volume. Thus, the majority of the lignin is located in the secondary wall. Furthermore, the lignin is uniformly distributed across the secondary wall in black spruce tracheids, as seen in Fig. IO. For more detailed information, the distribution of lignin in the xylem of Douglas fir [Pseudotsuga tnenziesii (Mirb.) Franco] is given in Table 10 [74]. It should be noted that the distribution of lignin in the various morphological regions of the tracheids is basically the same as that shown for black spruce in Table 9. For the ray parenchyma secondary wall, the lignin concentration is higher than that for the tracheid secondary wall but lower than that for the middle lamella. However, the secondary wall of the tracheids does not differ much from that of ray tracheids in its lignin Concentration. Table I I shows the distribution of lignin in loblolly pine (Pinus ruedcl L.) tracheids as determined by bromination coupled with SEM-EDXA [85]. One of the advantages of this techniquecomparedwith UV microscopy is the ability to study the S,, S,, and S, layers in the secondary wall as a separate entity. Such resolution is often difficult with UV microscopy. It is interesting to note that the lignin concentration in the S? layer is lower than that in either the S , or S, layer. The line profile of the bromine X-rays in Fig. 1 1 showssuch differences clearly. FukazawaandImagawa[89]havealsoreporteda similar finding of high UV absorbance near the lumen/wall interface for juvenile wood tracheids of Japanese fir (Abies suchalinensis Fr. Schm.). A comparison of Tables 9-1 1 shows that, minor differences not withstanding, the trends in the distribution of lignin in the tracheids of the three softwoods are similar. For the ray parenchymacellsconstitutingabout 5% of the total xylem tissue in softwoods, Harada and Wardrop[ 151 have reported a lignin content of 0.44 g/gin Japanese
TABLE 9 The Distribution of Lignin in Black Spruce Tracheids UV Microscopy
as
Determined by
~~
Lignin
Tissue Wood
Morphological volume region
(%)
(g/g) conc. (% of total)
~~~
Earlywood Latewood
S
87
72
0.23
ML ML,,
9 4 94 4 2
16
0.50 0.85
S
ML ML,, Source:
Ref. SO.
12 82 IO 8
0.22 0.60 1 .oo
67
Composition Chemical
FIGURE 10 UVphotomicrographtakenat 240 nm of theearlywoodtracheidwallsinblack spruce. The densitometer tracing was conducted along the dotted line. (Courtesy of Prof. Emer. D. A. 1. Goring, University of Toronto, Toronto, Canada.)
[66]obtained cedar (CryptorneriujuponicuD. Don). By a microdisection technique, Bailey a value of 0.41 g/g for the segregated ray parenchyma cells of Douglas fir. Fergus et al. [50] also determined byUV microscopy a lignin concentration of 0.40 g/g forblack spruce. These results by a variety of methods are in good agreement with the data shownin Table 10 for Douglas fir earlywood parenchyma cells. Interestingly, the ray parenchyma cellsin softwoods possess significantly higher lignin contents than the whole wood.
TABLE 10 The Distribution of Lignin in Douglas Fir Xylem as Determined by W Microscopy
Lignin
Tracheid
racheid
Tissue Wood
Earlywood ray ray Latewood ray ray Source: Ref. 74.
Morphological volume region S Tracheid ML Tracheid ML, Paren. S Tracheid S S
Tracheid ML Tracheid ML,, Paren. S Tracheid S
(%) (g/g)
conc.(% total)
74 10 4 8 4
58
0.25
18
0.56 0.83
90
78 10
0.40 0.28 0.23 0.6
6
0.9
4
-
4 2 3 1
11
10 3
2
Saka
60
TABLE 11 The Distribution of Lignin In Loblolly Pine Tracheids as Determined by Bromination with SEM-EDXA
Lignin
Tissue
wood Earlywood
Morphological volume region SI S2
S, ML
ML, Latewood
SI S2 S,
ML ML,
. (glg)
(%) conc total)(70of
13 60
9 12 6 6 80
5 6 3
12
0.25
44
0.20
9
0.28
21
0.49 0.64 0.23 0.18
14 6 63 6 14
0.25
0.5 1
11
0.78
Source: Ref. 85.
Regarding the distribution of lignin in the compression wood of softwoods, Timell [ 1l] has given an excellent review. As observed in an electron micrograph shown in Fig. 5 of the lignin skeleton from the compression wood of tamarack [Lark luricina (Du Roi) K. Koch], the S, layer appears to have a slightly lower lignin concentration than the inner S,. However,aringpresent in the S , layer [&(L)] reveals a high lignin concentration about equal to that in the middle lamella. Table 12 shows acomparisonmadebyTimell[l13 of theligninconcentrations determined by Wood and Goring 1741 of Douglas fir and by Fukazawa [90] of Japanese fir (Abies sachalinensis Fr. Schm.). Although the lignin content in Japanese fir is lower in most of the morphological regions, the overall trends are basically the same.
C
FIGURE 11 Scanning electron micrograph (a) of brominated latewood trachids in loblolly pine (0.5-pm section). The distribution map (b) of Br-L X-rays was taken of the same area as the scanning electron micrograph. The distribution of bromine (c) was taken along the line across the double cell wall. (From Ref. 83.)
69
Chemical Composition and Distribution TABLE 12 TheDistribution of LignininCompression Wood Tracheids of Douglas Fir and Japanese Fir
Morphological Douglasregion
Lignin concentration (%)
49
29 42 26 49
75
65
40 54 36
"From Ref. 14. hFrom Ref. 90.
C.
Distribution of Lignin in Hardwoods
Hardwood lignins consist mainly of guaiacyl and syringyl residues, and its ratio seems to change from one morphological region to another. Fergus and Goring [72,73] attempted to determine the distribution of lignin in white birch (Betula papyriferem Marsh.) byUV spectral analysis. The syringyl and guaiacyl residues have, however, markedly different UV absorptivities. Thus, it is essential to know its exact ratio before the lignin concentration in a particular morphologicalregion is computedfrom the UV microscopy. In the 1980s Saka et al. 191,921 developed a new method to compute the ratio of guaiacyl and syringyl residues at the various morphological regions by combining UV microscopy with bromination-EDXA (UV-EDXA). This could be used to determine lignin distribution in hardwoods. Shown in Table 13 is the ratio of guaiacylkyringyl residues in various morphological regions of white birch wood as determined by the UV-EDXA technique 1911. For com-
TABLE 13 Distribution of GuaiacylandSyringylResidues White Birch
in Lignin i n
Guaiacy1:syringyl
DXA Morphological omination" with region
uv analysish spectral Syringyl Guaiacyl Syringyl 5
0
Guaiacyl 50:50 5050
"From Ref. 9 1. 'From Ref. 73. 'Fiber/fiber. dFiber/vesscl. 'Fibedray. 'Ray/ray.
70
Saka
parison, the results obtained by Fergus and Goring [73] through UV spectral analysis are also included. It is indicated by both methods that the fiber secondary wall (S2) contains predominantly syringyl residues, whereas the vessel secondary wall (S?) consists mostly of guaiacyl residues. The study by UV-EDXA [91] revealed that the ray parenchyma cell contains about equalproportions of guaiacylandsyringylresidues in lignin. However,apredominant amount of syringyl-type lignin was found by UV spectral analysis [73], as in the fiber secondary wall. For the cell corner middle lamella (ML,,), 80-100% of the lignin was found to be guaiacyl residue, with the remaining 0-20% being syringyl residue by the UV-EDXA technique [91]. This result is not in agreement with the data by UV spectral analysis [73]. However, it supports the later suggestion of Musha and Goring [75]that the middle lamella lignin consists entirely of guaiacyl residues. Itis therefore apparent in Table 13 that, in hardwoods, the ratio of guaiacyland syringyl residues in lignin varies in different morphological regions. These findings have been supported by several investigators; Wolter et al. [93] have shown that the vessels in aspen callus cultures contain a pure guaiacyl lignin. Kirk et al. [94] found that the fungal degradation of lignin in birch wood was consistent withthe presence of syringyl-rich lignin in the fiber walls. Furthermore,Yamasakiet al. [95] isolated syringyl-rich lignin from several hardwoods. Hardell et al. [96] fractionated birch wood to determine the syringyl and guaiacyl ratio, and indicated that lignins in both the middle lamella and vessel secondary wall are rich in guaiacyl units, whereas the ratio of syringyl/guaiacyl residues is high in the fiber and ray cell. Cho et al. [97] studied the filmlike substance isolated from the fines of birch in which a high proportion of the compound middle lamella was recognized.This material wasfound to possessalow ratio of syringyl to guaiacyl units. Terashima et al. [98] administered 'H-labeled guaiacyl and syringyl model compounds to magnolia shoots and determined their location in the growing cell wall by microautoradiography. They found that the vessel wall, cell comer, and compound middle lamella were lignified by the deposition of guaiacyl-type lignin, and the fiber wall was composed of syringyl-guaiacyl lignin. Recently, UV and visible-light microscopic spectrophotometry have been combined with the Maule color reaction for detecting syringyl lignin by Yoshinaga [99], and this method has been extended to taxonomic studies of the distribution of hardwood lignins [ 100- 1021. Table 14 shows the distribution of lignin in white birch wood as determined by UVthe results obtainedearlier by UV microscopy 1721 are EDXA [91].Forcomparison, included. For the fiber secondary wall, the lignin concentration in the S, layer is slightly lower than in either the S , or S2 layer. However, its difference is so small that the lignin may be considered to be distributed uniformly across the secondary wall. The vessel walls also reveal a uniform distribution of lignin, but the concentration is about 1.9 times higher than that of the fiber walls, which in turn is higher than that of ray parenchyma cells. The cell comer middle lamella (ML,,) associated with fibers and vessels has the highest lignin concentration. In spite of sufficient analytical resolution by the EDXA system, the middle lamella between cell corner areas (ML) was 10-30% lower in concentration than the cell corner middle lamella (ML,,). It is of interest to note that the lignin concentration in the middle lamella regions of hardwoods is lower than that of softwoods, as seen in Tables 9 and 14. A comparison of the data made between UV-EDXA and UV microscopy techniques indicates that lignin concentrations in fiber and vessel secondary walls are in agreement
Composition Chemical
71
TABLE 14 The Distribution of Lignin in WhiteBirch
Element
Lignin concentration (g/g)
TissueMorphological volume region
(%)
11.4 58.5 3.5 5.2 2.4 1.6 4.3 2.3 0.8 =O
8.0 2.0 =O =O
UV-EDXA
uv only”
0.14
-
0.14 0.12 0.36 0.45 0.26 0.26 0.27 0.40 0.58
0.16
0.12
0.22
0.38 0.47 0.41
-
0.34 0.72 -
0.22 -
0.35 -
“From Ref. 9 1. hCalculated using xylem lignin content of 0.199 g/g; from Ref. 72. “Fiberlfiber. ‘Fiber/vessel. ‘Fiberlray. ‘Raylray.
with each other. However, the lignin concentration in the ray parenchyma cells byUVEDXA[91] is nearly half aslow as the dataobtained by UV microscopyalone[72]. Although the middle lamella between two cell corners (ML) of fibers and vessels revealed similar values by these two techniques, the concentration in the cell corner middle lamella (ML,,) was lower by the UV-EDXA technique [91]. The observed discrepancies are due probably to the uncertainty in estimating the guaiacyl/syringyl ratio, as the analysis is made by UV microscopy alone.
VI.
DISTRIBUTION OF INORGANIC CONSTITUENTS
A fair amount of information is available on the inorganic constituents of wood [1031091 and bark [ 110,ll l]. In woods from temperate zones, elements other than carbon, hydrogen, oxygen, and nitrogen make up between 0. l % and 0.5% of the weight of wood [ 1 12,1131, whereas those from tropical regions make up to 5% [ 1 141. This proportion, although small, contains a wide variety of elements. For example, spectrographic analysis of grand fir [l031 revealed as many as 32 elements (Table 15). In many cases, alkali and alkali earth elements such as Ca, Mg, and K make up about 80% of the total inorganic constituents [l 151. These elements probably occur in wood as salts, e.g., oxalates, carbonates, and sulfates [ 1161, or inorganic moiety bound to the cell wall components such as carboxyl groups of pectic materials [ 115,117,1181. Some of the inorganicelementspresent in wood are essential forwoodgrowth, whereas others are not necessarily required. Metalic elements are often absorbed into the tree through the root system and are transported to all areas within the growing tree [ 1031.
Sa ka
72
TABLE 15 Classification, Function, and Approximate Level of Occurrence of Elements Found in Wood of Grand Fir (ppm of dry weight)
Essential Major
Constituent C
Ca
754
0 H N P S
K Mg Na
865
c1
Si
171 23 -
B Mn
Fe
0.9 19.3 2.6
Ag 0.23 AI 5.4 Ba 20.2
MO
0.005
CO
Cu Zn
2.5 0.9
Cr Ni Pb Rb Sr
0.0 1 0.05 0.1 1 0.12 2.0 10.2
Ti
0.11
Au
0.04
0.02 Ga In La
0.03
Li 0.003 Sn
0.13
0.04
v
0.001
Zr
0.002
Source: Ref. 103.
For seven species, Young and Guinn [ 1091 have determined the distribution of 12 inorganic elements in various tissue areas of a tree such as the roots, bark, wood, and leaves. The results indicated that both total ash content and concentration of each element vary significantly within and between the species. Therefore, unlike major cell wall components such as cellulose and lignin, the content of inorganic constituents varies to a great extent with the environmental conditions under which the tree has grown [ 105,1131. Little has been published regarding the morphological distribution of elements in the cell [ 1 19- 1221. By microincineration, Lange [ 1 191 found that mineral constituents of Swedish spruce are deposited predominantly in the compound middle lamella. Zicherman and Thomas [ 1201 also have pointed out that careful ashing of microtome sections of loblolly pine (Pinus r n e h L.), followed by electron microscopic observations, gives an ash residue distributed throughout the cell wall and concentrated in the compound middle lamella and S, layer. Wultsch [ 1211 stated that manganese is concentrated in ray cells, and Bergstrom [ 1221 reported that the phosphoruscontent is highest in the cambiumandadjacentxylem portions. Saka and Goring [ 1151 have studied the distribution of inorganic constituents from the pith to the outer ring of black spruce (Picea nznriann Mill.) by means of TEM-EDXA. The TEM-EDXA technique is a useful tool fordetectinganyelementaboveneonand recently above boron in the periodic table. Figure 12 shows seven morphological regions of the tracheids, ray tracheids, andrayparenchymacells investigated. Thedarkcircle indicates the location of the analysis and its diameter corresponds to the resolution of analysis (400 nm). Detected were 15 different elements, such as Na, Mg, AI, S, Cl, K, Ca, Cr, Fe, Ni, Cu, Zn, and Pb, above neon in the periodic table. The secondary walls of tracheids, ray tracheids, and ray parenchyma cells usually contain detectable concentrations of only four elements: sulfur, chlorine, potassium, and calcium. In contrast, almost all the elements were found to be localized and concentrated in the torus and half-bordered pit membrane regions (Fig. 13). The total content of inorganic constituents decreased in the order of torus (2%) > half-bordered pit membrane (1%) > middle lamella (0.4%) > ray parenchyma cell wall (0.3%) > tracheid secondary wall (0.1-0.15%). The total content of inorganic constituents was higherin earlywood than latewoodfor any of the morphological
omposition Chemical
and Distribution
73
FIGURE 12 Transmission electron micrographs of a cross section of black spruce showing the seven different morphological regions. All micrographs were takenat the same magnification. S , = secondary wall of the tracheid CC = cell comer middle lamella surrounded by tracheids TT = tours in an intertracheid pit pair SR = secondary wall of the ray parenchyma cell M = a half-bordered pit membrane between ray parenchyma cell and tracheid SRT = secondary wall of the ray tracheid TRT= torus in an intertracheid pit pair between ray tracheid and tracheid
74
Saka
FIGURE 13 EDXA spectra from the tracheid secondary wall and tracheid torus in black spruce. (From Ref. 115.)
regions studied. This is probably because the earlywood tracheids that have large lumens and abundant pits are the major water-conducting tissues, whereas thick-walled latewood tracheids with fewer pits may act as a physical or mechanical support for the wood. Bailey and Reeve [l231 have recently used imaging microprobe secondary ion mass spectrometry (SIMS) to determine the distribution of the trace elements in black spruce (Picea rnariana Mill.). This imaging microprobe S N S technique is a powerful tool for detecting inorganic elements with high spatial resolution and high sensitivity. Their overall findings correlatewell with results from the TEM-EDXA studyby Saka and Goring[ 1151. However, due to its higher sensitivity compared with the EDXA technique, the distribution of the elements within the cell wall could be more clearly demonstrated. Figure 14 is one example in which some elements are visualized and concentrated in the middle lamella region. Recently, Saka and Mimori [l241 have studied the distribution of inorganic constituents of Japanese birch wood (Betula platyphylla Sukatchev var. Japonika Hara) by the SEM-EDXA technique with thin sections. Figure 15 shows six morphological regions of the fibers, vessels, and ray parenchyma cells investigated. The dark circle corresponds to the resolution of analysis (800 nm). Detected were 11 different elements: Na, Mg, Al, Si, P, S, Cl, K, Ca, Fe, and Zn. The secondary walls of wood fibers, vessels, and ray parenchyma cells usually contained detectable concentrations of three elements, S, Cl, and Ca, while, in the amorphous layer of ray parenchyma cell and pit membrane between vessel and ray parenchyma cell, almost all of the detected elements were found to be localized and concentrated (Fig. 16). The total content of inorganic constituents decreased in the order amorphous layer (0.68%) > fiber middle lamella (0.54%) > vessel middle lamella
Composition Chemical
75
FIGURE 14 Ion image and its intensity for Ca. Fe, and Mn from a tangential section of a double cell wall of black spruce heartwood. (Courtesy of Prof. D. W. Reeve, Universityof Toronto, Toronto, Ontario, Canada.)
> fibersecondary wall (0.14%) > vessel (0.48%) > ray parenchema cell wall (0.15%) secondary wall (0.10%).This observed trend is basically the same as found in black spruce by Saka and Goring [115]. VII.
CELL WALL ORGANIZATION
In the previous sections, current knowledge of the distribution of cell wall constituents was described. In this section, therefore, how these constituents construct and organize the cell wall structure is discussed. In wood cell walls, cellulose acts as the structural framework in the formof cellulose microfibrils, while hemicellulose is the matrix substance present between these microfibrils. Lignin, on the other hand, is the encrusting substance binding the wood cells together and giving rigidity to the cell wall. Generally, the S2 layer increases with increasing wall thickness, whereas the S , and S , remain fairly constant. Because of its greater thickness, the S2 layer is largely responsible for the physical and mechanical properties of the cell walls. Figure 17 shows the relationship for softwoods between the lignin content and microfibrillar angle (e) in the tracheid S2 layer determined by the X-ray diffraction method. Since the majority of the lignin in softwoods is in the tracheid S , layer [50], the whole lignin content of wood must be closely correlated to the lignin concentration in the S , layer of the tracheid. Thus, from Fig. 17, the lignin concentration in theS , layer increases
76
Saka
c
FIGURE 15 Scanning electron micrographs of a transverse section of the Japanese birch wood showing the six different morphological regions considered in this study. Fs = secondarywall of thewoodfiber F,, = cell comer middle lamella surrounded by wood fibers Vs = secondarywall of thevessel VML= cell comer middle lamella surrounded by vessel and wood fibers Rs = secondarywall of therayparenchymacell RA, = amorphous layer in the ray parenchyma cell
with increasing microfibrillar angleof the tracheid S2 layer [ 1251. The biosynthetic origin
of this relationship is not known. However, it does suggest that, in order to construct the enforced plywood type of structure shown in Fig. 1, the three major chemical constituents of wood mutually interact and strengthen each other to make up a natural supercomposite material. Figure 18 shows such an ultrastructural arrangement of cellulose microfibrils, hemicellulose, and lignin in wood cell walls as proposed by Harada and CBtC [126]; around the core of cellulose microfibrils, paracrystalline regions of cellulose are thought to exist, which are associated with hemicellulose and lignin. Lignin encases them and binds them into the rigid structure of the wood cell wall. At the molecular level of arrangement of the chemical composition, the presence of a chemical bond between lignin and carbohydrate has been proved to be a lignin-carbohydrate complex (LCC) [l271 which is considered to be a compatibilizer-like substance localized at the interface between hydrophobic macromolecules of lignin and hydrophilic carbohydrates, by enhancing the physical and mechanical properties of wood [128].
77
Chemical Composition and Distribution
I
.
D-
4
I
I
FIGURE 16 Scanning electron micrograph (a) of a cross section of Japanese birch. The arrow shows the location of the EDXA analysis at the pit membrane between vessel and ray parenchyma cells from which the EDXA spectrum (b) was obtained.
45
2
40
Y
c
c
2 35 S
c *g 30 3
25 20 0
10 5 020 4 0 3 0 Microfibrillar angle Cel
FIGURE 17 Relationshipbetweenthemicrofibrillarangle lignin content of wood. (From Ref. 125.)
(e) inthetracheid
S2 layerandthe
78
Saka
FIGURE 18 Schematic diagram of the ultrastructural arrangement of a cellulose microfibril (Mf), hemicellulose (H), and lignin (L) in the wood cell wall. (From Ref. 126.)
VIII.
CONCLUDINGREMARKS
Knowledge of the chemical composition of woodis essential for studying the physical and chemical properties of wood. However, it can provide nothing but the average of the cell wall constituents. For a better understanding of wood properties, more detailed information is required about their distribution across the wood cell wall. However, in spite of a variety of methods proposed, all the methods have drawbacks and thus some discrepancy exists among investigators. A good method for resolving such discrepancies would be to separatevarioustypes of tissues physicallywithoutintroducinganychemicalchanges [49,96]. Analysis of the separated tissues could then provide definitive information on the distribution of the cell wall constituents at the various morphological regions of wood.
REFERENCES 1.
2. 3.
4. 5.
6.
7. 8. 9. 10. 11.
12. 13. 14.
A.B.Wardropand D. E. Bland, in Biochemistry of Wood (K. Kratzland G. Billek, eds.), Pergamon Press, London, p. 92 (1959). H. Harada, Mokuzai Gakkaishi, 30:513 (1984). F.F.P. Kollmann and W.A. C M , Jr., Principles of Wood Science and Technology, Vol. I, Solid Wood, Springer-Verlag, Berlin, p. 43 (1968). B. L. Browning, The Chemistty of Wood, Wiley-Interscience, New York, p. 57 (1963). T. E. Timell, in Cellular Ultrastructure of Woody Plants (W. A. CBtC, Jr., ed.), Syracuse Univ. Press, New York, p. 127 (1965). H. Meier, in Biosynthesis and Biodegradation of Wood Components (T. Higuchi, ed.), Academic Press, New York, p. 43 (1985). F.F.P. Kollmann and W. A. CBtC, Jr., Principles of Wood Science and Technology, Vol. I, Solid Wood, Springer-Verlag, Berlin, p. 55 (1968). W. A. C M , Jr., in Recent Advances in Phytochemistry, Vol. 11 (F. A.Loewusand V. C. Runeckles, eds.), Plenum Press, New York, p. 1 (1977). T. E. Timell, Wood Sci. Technol., 1:45 (1967). H. Higuchi, KASEAA, 13:206 (1975). T. E. Timell, Wood Sci. Technol., 16233 (1982). G. Schwerin, Holdorsch., 12:43 (1958). M. Fujii, J. Azuma, F. Tanaka, A. Kato, and T. Koshijima, Wood Res., 68:8 (1982). G. C. Hoffmann and T. E. Timell, Tappi, 55:733 (1972).
Chemical Composition and Distribution
79
15. H. Harada and A.B.Wardrop, MokuzaiGakknishi, 6:34 (1960). 16. 0. Perila, J. Pol.ymer: Sci., 51:19(1961). 17. 0. Perila and P. Heitto, Suomen Kemistilehti, B32:76 (1959). 18. G. C. Hoffmann and T. E. Timell, Tappi, 55:871 (1972). 19. H.Meier, Pure Appl. Chem., 5:37 (1962). 20. P. Whiting and D. A. I. Goring, Post-Grad. Res. Lab. Rep. 241, PPRICAN, Quebec, Canada (1981). 21. W. A. C8t6, Jr., N. P. Kutscha, B. W. Simson, and T. E. Timell, Tnppi, 51:33 (1968). 22. W. A. C M , Jr., A. C. Day, N. P. Kutscha, and T. E. Timell, Holz&rsch., 21: 180 (1967). 23. R. B. Hanna and W. A. C8t6, Jr., Cytobiologie, 1 0 1 0 2 (1974). 24. T. Goto, Ph.D. thesis, Dept. Wood Science Technology, Kyoto Univ., Kyoto, Japan (1976). 25. A. N. J. Heyn, Tippi, 60:l59 (1977). 26. G. Cox and B. Juniper, J. Microscopy, 97343 (1973). 27. J. B. Boutelje and B. H. Hollmark, Hol$orsch., 26:76 (1972). 28. V. M. Sinner, N. Parameswaran, H. H. Dietrichs, and W. Liese, Hol$orsch., 2 7 3 6 (1973). 29. M. N. Sinner, N. Parameswaran, N. Yamazaki, W. Liese, and H. H. Dietrichs, Appl. Polymer: Symp., 28:993 (1 976). 30. P. Hoffmannand N. Parameswarm, Holdorsch., 30:62 (1976). 3 1. T. Awano, K. Takabe, and M. Fujita, Abstr: 46th Annual Meeting of the Japun Wood Resenrch Society, p. 32 (1996). 32. T. Fujii, H. Harada, and H. Saiki, MokuzniGakknishi, 27:149 (1981). 33. W. A. C M , Jr., A. C. Day, and T. E. Timell, Wood Sci. Technol., 2 : I3 (1968). 34. N. Parameswaran and W. Liese, Holz.Roh.-Werkst.. 40:145 (1982). 35. P. Albersheim, K. Muhlethaler,and A. Frey-Wyssling. J. Biophys. Biochem. Cyrol., 8501 ( 1 960). 36. R. M. McCready and R. M. Reeve, Agric. Food Chem., 3:260 (1955). 37. M. Gee, R. M. Reeve, and R. M. McCready, Agric. Food Chem., 7 3 4 (1959). 38. E. M. Barmicheva and M. F. Danilova. Bo?.Zh., %':l278 (1973). 39. P. M. Colombo and N. Rascio, J . Ultrustruct. Res., 60:135 (1977). 40. Y. Czaninski, Biol. Cellulnire, 35:97(1979). . R389 (1936). 41.A. J. Bailey, lnd. Eng. Chem., A I Z U ~Ed., 42. H. Meier, J. Polymrc Sci.. 5 / :1 1 (1961 ). 43. H. Meierand K. C. B.Wilkie, Hol
80
Saka
61. H. Meier, Holz Roh-Werkst., 13:323 (1955). 62. I. B. Sachs, 1. T. Clark, and J. C. Pew, J . Polymer. Sei. Part C, 2:203 (1963). 63. A. L. K. Bentum, W. A. CGtC, Jr., A. C. Day, and T. E. Timell, Wood Sei. Technol., 3:218 ( 1969). 64. R. A. Parham and W. A. CGtC, Jr., Wood Sei. Technol., 5:49 (1971). 65. P.W. Lange, Svensk Papperstidn., 57525 (1954). 66. A. J. Bailey, Ind. Eng. Chem., Anal. Ed., 8 5 2 (1936). 67. G. J. Ritter, Ind. Eng. Chem., 17:1 194 (1925). 68. J . A. N. Scott, A. R. Procter, B. J. Fergus, and D. A. I. Goring, WoodSei.Technol., 3:73 ( 1969). 69. J. A. N. Scott and D. A. I. Goring, Wood Sei. Technol., 4:237 (1970). 70. J. R. Wood and D. A. 1. Goring, J. Microsc., 100:105 ( 1 974). 71. J . A. N.Scott and D. A. I. Goring, Cell. Chenz. Technol., 4:83 (1970). 72. B. J. Fergus and D. A. 1. Goring, Hollforsch., 24: I 18 ( 1970). 73. B. J. Fergus and D. A. I. Goring, Hollforsch., 24: 1 13 (1970). 74. J. R. Wood and D. A. I. Goring, Pulp Paper Mag. Can.,72:T95 ( 1971 ). 15. Y. Musha and D. A. 1. Goring, Wood Sci. Technol.. 9 4 5 (1975). 76. G. P. Berlyn and R. E. Mark, Forest Prod. J., 16:140 (1965). 77. J. M. Yang and D. A. I. Goring, Pulp Paper Can. Trans., 4:2 (1978). 78. J. M. Yang and D. A. I. Goring, Can. J. Chem., 58:2411 (1980). 79. P. Whiting and D. A. I. Goring, Paperi j a Puu, 10592 (1982). 80. P.W. Lange and A. Kjaer, Norsk Skogind, 11:425 (1957). 81. J. B. Boutelje, Svensk Papperstidn., 75:683 (1972). 82. S. Saka, R. J. Thomas, and J. S. Gratzl, Tcppi, 6l:73 (1978). 83. S. Saka, R. J. Thomas, and J. S. Gratzl, Proc. ISWPC, Stockholm, Sweden, Vol. I , SPCI Rep. 38, p. 35 (1981). 84. S. Saka and R. J. Thomas, Wood Sei. Technol. 16:1 ( I 982). 85. S. Saka and R. J. Thomas, Wood Sci. Technol., 16:167 (1982). 86. S. Saka, P. Whiting, K. Fukazawa, and D. A. I. Goring, Wood Sci. Technol., 16:269 (1982). 87. U. Westermark, 0. Lidbrandt, and 1. Eriksson, Wood Sci. Technol.. 22:243 (1988). 88. I. Eriksson, 0. Lidbrandt, and U. Westermark, Wood Sei. Echnol., 22:25 1 ( 1988). 89. K. Fukazawa and H.Imagawa, Wood Sei. Technol., 15:45 ( 1981). 90. K. Fukazawa, Res. Bull. Coil. Exp. Forests Hokkaido Univ., 31:87 (1974). 91. S. Saka and D. A. I. Goring, Hollforsch., 42: 149 ( 1988). 92. S, Saka, S. Hosoya, F. G. T. St-Germain, and D. A. I. Goring, Holiforsch., 42:79 ( 1988). 93. K. E. Wolter, J. M. Harkin, and T. K. Kirk, Physiol. Plartt, 31: 140 (1974). 94. T. K. Kirk, H.-m. Chang, and L. F. Lorenz. Wood Sei. Technol., 9 8 1 (1975). 95. T. Yamasaki, K . Hata, and T. Higuchi, Hollforsch.. 32:44 (1978). 96. H.-L. Hardell, G . J. Leary, M. Stoll, and U. Westermark, Svensk PqJperstidn.,83:71 (1980). 97. N. S. Cho, J. Y. Lee, G. Meshitsuka, and J. Nakano. Mokuwi Gakkcrishi, 26:527 (1980). 98. N. Terashima, K. Fukushima. and K.Takabe, Hol;for.sch., .CO(Suppl.):lOl (1986). 99. A. Yoshinaga. Ph.D. thesis, Dept. Wood Science Technology, Kyoto Univ., Kyoto,Japan ( 1995). 100. K. Takabe, S. Miyauchi. R. Tsunoda, and K. Fukazawa. IAWA Bull., I Z . ~ . 1, 3 : 105 ( 1992). 1 0 1 . J. Wu. K. Fukazawa. and J. Ohotani, Hol&rseh., 46:181 (1992). 102. Y. Watanabe and K. Fukazawa, Res. Bull. Hokknido Uni1: Forests, 50:349 ( 1 993). 103. E. L. Ellis, in Cellulrr Ultrastructure cf Woo& Pltrrrts (W. A. CGtC, Jr., ed.), Syracuse Univ. Press, New York, p. 18 1 ( 1965). 104. R. F. Dyer, Tech. Bull. No. 27, Univ. Maine, Maine Agric. Exp. Sta. (1967). 105. E. L. Ellis, Forest Prod. J., 12:271 (1962). 106. W. L. Galligan, H. Stern, and P. Hohenschuh, Forest Prod. J., 15:185 (1965). 107. H. E. Young and P. W. Carpenter, Tech. Bull. No. 28, Univ. Maine. Maine Agric. Exp. Sta. ( 1967).
omposition Chemical 108.
109. 1 IO. 111. 112.
113.
114. 1 15.
116. 117. 118.
119. 120.
121. 122. 123.
124. 125.
126. 127. 128.
81
H, E. Young, P. N. Carpenter. and R. A. Altenberger. Tech. Bull. No. 20, Univ. Maine, Maine Agric. Exp. Sta. (1965). H. E. Young and V. P. Guinn, Rrppi, 49:190 (1966). M. L. Harder and D. W. Einspahr, Tappi. 63:110 (1980). H . E. Young. Forest Prod. J., 2 / 5 6 (1971). A. J . Panshin and C. de Zceuw, Te.srbook of Wood Techrwlogy, 3rd ed., Vol. l , McGraw-Hill, New York, p. 73 (1970). B. L. Browning. The Chenlisfry of Wood, Wiley-Interscience, New York, p. 355 (1963). J. Savard, J. Nicolle, and A. M. Andre, Analyse chimique des bois tropicaux, Centre Technique Forestier Tropical. Nogent-sur-Marne (1960). S. Saka and D. A. I. Goring, Mokuzcri Gakkcrishi, 29:648 (1983). E. T. Choong, G. Abdullah, and J. Kowalczuk, LSU Wood Uti1i:utiorl Notes No. 24, (1976). B. E. Cutter, E. A. McGinnes, Jr.. and D. H. McKown, Wood Fiber, 12:72 (1980). H. Wazny and J. Wazny. Hol: Rol~-Werkst.,22:299 (1964). P. W. Lange. Pulp. Ptrper Mcrg. Carl., 59:2 10 (1958). J. B. Zicherman and R . J. Thomas, firppi, 54:1727 (1971). F. Wultsch, P ~ p e rFc11x. 4: 128 ( 1944). H. Bergstriim, S ~ w z s kPcrpper.stidn.. 62:160 (1959). J. H. E. Bailey and D. W. Reeve, J . Pulp Prrper Sci., 20:J83 (1994). S. Saka and R. Mimori, M o k w a i Gakknishi, 40:88 (1994). S. Saka and M. Tsuji, Cellulose Clwm Teclmol.. 2/:225 (1987). H. Harada and W. A. C6t6, Jr.. B i o s p t h e s i s and Biodegradation of Wood Co,nponer~f.s, p. 20, Academic Press, New York (1985). T. Koshijima, Wood Res. Tech. Nores, 19:1 1 (1984). S. Takase, N. Shiraishi. and M. Takahama, Wood Processing and Utilizcrtion, p. 243, Wiley, Chichester. U.K. (1989).
This Page Intentionally Left Blank
Structure of Cellulose: Recent Developments in Its Characterization Furnitaka Horii Kyoto University, Kyoto, Japan
1.
INTRODUCTION
The first Laue X-ray diffraction photographs of native cellulose, such as ramie and bamboo, were taken by Nishikawa and Ono in 1913 [l]. Since then a lot of effort has been madetocharacterize the crystal structure of nativecellulose,mainlyusing the X-ray diffraction technique. Nevertheless, the detailed structure has not been clarified as yet, and the reason for the difficulty has only recently been understood reasonably. Although it was assumed in the traditional analyses that native cellulose was composed of single homogeneous crystals, this assumption has been found not to be fulfilled in most specimens from different native sources: native cellulose crystals have been confirmed to be composites of at least two types of crystal allomorphs. This chapter deals with the process of theconfirmation of such a new crystal structuremodelfornativecellulosesomewhat historically. Further recent developments relating to this model of crystallization are also described by focusing attention on cellulose biogenesis by a bacterium. For other progress in characterization of cellulosic materials, refer to recent review articles [2-41.
II. COMPOSITE CRYSTAL MODEL Since the first observation of CP/MAS I3C NMR spectra of native celluloses in 1980 [5,6], it has been recognized that there are great differences in multiplicities of the Cl and C4 resonance lines between two groups, the bacterial-Vrtlorziu group and the cotton-ramie group. Figure 1 shows CP/MAS I3C NMR spectra of the crystalline components of these native celluloses [7,8], which were selectively measured by using longer "C spin-lattice relaxation times (TIC)of the components[9,10]. Asis readily seen,cotton and ramie celluloses give almost the same crystalline spectrum, whereas bacterial and klonia celluloses produce a different type of crystalline spectrum. The most prominent features of these two types of crystalline spectra appear in the C1 resonances; a predominant doublet with a weak central singlet is observed for cotton and ramie celluloses, while a triplet composed of an enhanced singlet and a minor doublet appears for bacterial and Valonia celluloses. These fine splittings, including those in the C4 and C6 lines, should be due to 83
a4
Horii
120
IIIIIIII,,I,,,II,,,,1,,,~I,,,,l,,,,I,,,,I,,,,I,,,,I,,I,I,,,,I,,,,I, 110 10 0 90 80 70 60 50
P m
from TMS
FIGURE 1 CP/MAS "C NMR spectra of the crystalline components included in differcnt native celluloses: (a) cotton; (h) ramie; (c) bacterial; (d) Vcrlorzicc celluloses 171.
the existence of carbon nuclei in magnetically nonequivalent states. It is therefore suggested that there must be significant differences in conformations around the 1,4-glycosidic linkage and the C5-C6 bond, hydrogen bonding, or molecular packing between the two groups. Nevertheless, it should be noted that the relative intensities of the C 1 and C4 lines are not described i n terms of small whole numbers, as would be expected if they arose fro111 different sites within a single unit cell. Similar structural differences between these two groups were also suggested by mea-
Structure of Cellulose
a5
surements of IR spectra about 40 years ago [ 1 l]; the absorption bands due to stretching of OH and CH groups were markedly different between the bacterial-Vulonia group and the cotton-ramie group. A separate electron diffraction study [ 121 also proposed that the so-called eight-chain unit cell was appropriate to interpret the diffraction pattern observed for Vuloniu cellulose, whereas the diffraction spots for ramie and cotton celluloses were usually indexed in terms of the Meyer-Misch-type two-chain unit cell. In the 1970s more detailed structural analyses were also carried out by wide-angle X-ray diffractometry [ 13151. However, these important efforts did not lead in a straightforward way to the idea that native cellulose crystals are composed not of single pure crystals but of a mixture of crystals with different crystal forms. In 1984,AtallaandVanderHart [ 16,171 proposed by their careful elucidation of CPMAS l3C NMR spectra of different native celluloses that native cellulose crystals are composites of two allomorphs that are referred to as cellulose I, and cellulose I,. This proposal, which should be estimated as an epoch-making contribution to the enhancement ofnew effortstoward the structural characterization of nativecellulose,wasmade by showing that the individual resonance lines were obtained by appropriate linear combinations of the spectra of the regenerated cellulose I that contains almost the pure I, form and bacterial cellulose that is rich in the I, form. Figure 2 shows schematically the spectra of the C, and C, carbons thus obtained for celluloses 1, and I, [16-181. The I,, form has singlets for the C l and C6 carbons and a doublet for the C4 carbon, whereas the I, form has doublets for the C l , C4, and C6 carbons. The multiplicities in the I, and I, spectra are reasonably interpreted by the structural inequivalences in single unit cells, in contrast to those in the whole spectra as described in Fig. 1. However, the novel structural model thus proposed, which is hereafter referred to as the composite crystal model, was not readily established, because the relative intensities of the C l and C4 triplets could not be fully interpreted by this model for different native celluloses [7], suggestingthe existence of some exceptions depending onthe native sources of celluloses. For example, Fig. 3 shows the results of lineshape analysis of the C4 resonance lines for native celluloses with higher contents of cellulose I,, [ 191. The most upfield line, which would be described by a single Lorentzian curve according to the composite crystal model, are found in this case to be composed of two Lorentzians with different intensities for these cellulose samples. In such a situation we need additional experimental evidence to support the composite crystal model.
111.
CRYSTAL TRANSFORMATION FROM CELLULOSE I, TO CELLULOSE I,
There maybe someways to confirm the composite crystal modelexperimentally.For example, one way is to collect native celluloses having more widely different I,, and I, contents, particularly to find native cellulose with much higher I,, content or the pure I,, form. Since this may be awfully time-consuming work, we tried to find a route to induce the crystal transformationbetweencelluloses I,, and I,. The fourfollowingcaseswere found to induce the crystal transformation from cellulose I,, to I,: l . Annealing at hightemperatureswith saturated steam [20] 2 . Annealing at hightemperatures in alkaline aqueous solutions [21] 3 . Solid-stateregenerationfromcellulose triacetate I [22] 4. Solid-stateregenerationfromcellulose 111, [23]
Horii
c1
c4
cellulose I a I
I
I
I
I
I
I I
I I
I I
1.j1 Ill I
cellulose t
I I
I I
i
I
h! I
cellulose I g
The first treatment was developed originally from the steam explosion of wood, by carefully elucidating the experimental fact that CP/MAS "C NMR spectra of Japanese birch and cypress were greatly changed before and after steam explosion at 255°C [24]. However, drastic degradation of cellulose occurs with saturated steam at 255°C when the samples are not wrapped with glass fiber sheets. Such degradation Inay be induced by the effect of hydrogen ions that are produced by the much higher level of the dissociation of water at higher temperatures. Considering this situation, influences of the pH values of aqueous nledia were investigated at different temperatures. Finally, annealing was found
87
Structure of Cellulose
,
92
90
.
1
R8
.
,
X6
1
92
,
I
90
.
I
88
,
l
X6
i
,
92
I
,
I
.
I
90
86 ppm from TMS
FIGURE 3 Lineshape analyses of the C4 resonance lines for Valonia mncrophyscr (a), Cladophonr (b), and bacterial (c) celluloses [19].
to be most effectively carried out in a 0. I N NaOH aqueous solution at 260-280°C without significant degradation [21]. Figure 4 shows CP/MAS I3C NMR spectra of Valotzicc macrophysa cellulose and its annealed samples at 220-280°C for 30 min in the 0.1 N NaOH aqueous solution [ 171. The enhanced central line of the C l triplet of the intact sample, which is one of the features for Itr-rich samples, is greatly reduced in intensity with increasing annealing temperature, whereas the doublet at both sides is concomitantly increased in intensity. The C4 triplet is also transformed into a doublet as a result of the reduction of the most downfield line and the concomitant increase of the most upfield line. The C6 resonance line is also a triplet with minor separation, and almost the same change in lineshape as the C l triplet is induced by the annealing. Finally, the C I , C4, and C6 resonance lines are all doublets, which is in good accord with the spectrum proposed for cellulose I, as shown in Fig. 2 . All the C l and C4 resonance lines shown i n Fig. 4 were successfully interpreted in terms of the linear combination of the spectra for celluloses I,, and I, shown in Fig. 2 [ l 81. The mass fraction of cellulose I,, that was determined by the lineshape analysis of the C l and C4 resonances 181 is plotted against the annealing temperature in Fig. 5. Here, the results obtained by annealing under high pressure are also shown. I t is clearly seen that almost all cellulose I,, is transformed into cellulose I, by the annealing, because there is almost no change in the total degree of crystallinity in this treatment. In addition, the appearance of the microfibrils also undergoes no change, indicating almost perfect crystal transformation occurring in this system. Organic solvents such as ethylene glycol, ethyl alcohol. and monoglyme and helium gas are also effective in inducing the crystal transformation from cellulose I,, to l,,, but the efficiency is not so high compared to the cases of saturated steam and alkalineaqueous solution (251. In the cases of generation from cellulose triacetate I and cellulose 111, there were significant decreases i n crystallinity and apparent splaying of the microfibril structure (22,231. Electron diffraction analysis also confirmed the crystal transformation from cellulose l,, to I,. Figure 6 shows electron diffraction diagrams of delaminated Vrrlor~icrrt~crcrq~hyscr fragments before and after annealing in the 0.1 N NaOH aqueous solution [26].The diffraction diagram of the original sample. which is identical with the patterns previously published. has triclinic character, particularly on the third layer line. In Fig. 7 is shown the densitometer traces of the third-layer lines for the samples annealed at different temperatures. The reflections occurring at the left-hand side of the meridian have different intensities from those at the right-hand side for the original Krlorzitr cellulose. Such triclinic features are drastically changed with increasingannealingtemperature. Finally. the dif-
88
Horii
c1 C 2.3.5
l r
Y
100 60
80 ppm from T M S
FIGURE 4
CPA4AS I3C NMR spectraof k / o r l i < l macrophysa celluloseannealed at different temperatures in 0.1 N NaOHaqueoussolution:(a)original; (b) 220°C; ( c ) 240°C; (d) 260°C; (e) 280°C [ 181.
Structure of Cellulose 0.
1
1
1
89 1
1
I
I
1
I
t 1
0 Annealing temperature /'C
FIGURE5 The mass fraction of cellulose I, as a function of annealing temperature when annealed in 0.1 N NaOH aqueous solution: (A) under saturated steam pressure; (0)under 5 kbar.
fraction diagram becomes completely symmetric for the sample annealed at 260°C, indicating monoclinic character. It was also found that all spots shownin Fig. 6C are indexed with a two-chain P2, unit cell with a = 0.792 nm, b = 0.822 nm, c = 1.036 nm, and y = 97.3", whilethecorrespondingspotsshown in Fig. 6Aareindexedwithatwo-chain triclinic unit cell with a = 0.954 nm, b = 0.825 nm, c = 1.036 nm, a = 90°, p = 57.0", y = 96.6". It is therefore concluded that cellulosesI, and I, should be assigned to the twochaintriclinicandmonoclinicphases,respectively.However, the more stable form of cellulose I, can be assigned to the one-chain triclinic phase, as described later. Similar structural changes by annealing are also recognized by FT-IR spectroscopy. Figure 8 shows the FT-IR spectrum of Rhizoclonium cellulose before and after annealing in the 0.1 N NaOH aqueous solution [27]. Two absorption bands are clearly observed at 3240 and 3270 cm" in the OH stretching region and also at 750 and 710 cm" in the CH2 rocking region for the original sample, but the former bands almost disappear after annealing. This fact clearly indicates that the former bands are assignable to cellulose I,, whereas the latter bands can be ascribed to cellulose I,. Moreover, it may be suggested
FIGURE 6 Electron diffraction diagrams of Vuloniu cellulose before andafter its annealing: A, original; B, annealed at 240°C; C, annealed at 260°C [26].
90
Horii mer i d i a n
I
l
I
I
0
.2
I
.4
R FIGURE 7 Densitometer traces of the third layers of the electron diffraction diagrams for Valonia cellulose annealed at different temperatures: (a) control; (b) 220°C; (c) 240°C; (d) 260°C.
L
4000
3600 3200 2800 2400
wavenumber (cm-') FIGURE 8
1000
800
600
400
wavenumber (cm-')
FT-IR spectra o f original (A) and annealed (B) Khi:oc.lorliltr?! cellulose 127)
Structure of Cellulose
91
that the hydrogenbondingassociatedwith the CH,OH group is significantly different between the two allomorphs, in good accord with the finding by Raman spectroscopy [28]. Using the bands in the CH, rocking region, we developed a more convenient method to determine the mass fraction of cellulose I, or I, compared to the solid-state "C NMR method described above. In this case lineshape analyses of FT-IR spectra and CPMAS I3C NMR spectra were carried out at the same time for Valonia and bacterial celluloses annealed at different temperatures. Then the following equation was obtained between the mass fraction f F of cellulose I, determined by FT-IR and the mass fraction f t"" estimated by solid-state "C NMR [29]:
ft"" = 2.55f:
- 0.32
r"")
of cellulose Since this equation is a sort of calibration curve, the mass fraction f , (=f I, can be determined by FT-IR spectroscopy using a specimen of the order of milligrams.
IV.
DISTRIBUTION OF CELLULOSES I, AND I, IN NATURE
Figure 9 shows mass fractions of cellulose I, of representative native celluloses, which were determined by C P M A S I3C NMR or FT-IR spectroscopy. Marine algal and bacterial cellulosesarefound to be rich in cellulose I,; the average fraction is about0.63.For example, its value is 0.64 for Valonia rnacrophysa, 0.60 for Valonia aegurropilu, 0.67 for Chaetornorpha, and0.65 for Cladophora. In the case of bacterial cellulose, the mass fraction of cellulose I, depends on strains and culture temperature, ranging from 0.64 to 0.71. Careful purification with aqueous alkaline solution will reduce the content of cellulose I, by several percent for bacterial cellulose. On the other hand, cellulose-forming cell walls of higher plants such as cotton and ramie are rich in cellulose I,, the mass fraction being about 0.8. When these native celluloses, including algal and bacterial celluloses, undergo annealing at high temperatures, their I, fractions all increase up to about 0.9, but there is still some contribution from the I, phase. Since such a minor contribution cannot be detected by electron diffractometry, the size of the crystallites of the residual I, form must be significantly small. In nature, however,almostpurecrystals of the I, formcanbeobtainedfrom tunicate cellulose
valonia, bacterial
I-
-
L-
cotton, ramie annealed
tunicate
FIGURE 9 Distribution of the mass fraction of cellulose I,, in nature [ 191.
Horii
92
[21,30]. In contrast, it is still impossible to obtain the pure l,, form in nature and also by any artificial method at present. As for the characterization of woods, there is normally a difficulty in exact I3C NMR measurements of the crystalline component because of the low crystallinity and the coexistence of hemicelluloses and lignin. However, our recent CP/MAS "C NMR analysis has clearly revealed that normally lignified woodcellulose in Populus muxomowiczii, which belongs to hard woods, is cotton-ramie type, the mass fraction of cellulose I, being estimated to be about 0.8 1311. This result seems to be in conflict with our preliminary results for Japanese cypress and birch [24], in which cellulose I,, was assumed to be rather dominant. Recently, Newman measured separately the CP/MAS "C NMR spectrum of the cellulose component as a result of the removal of the contributions from hemicelluloses and lignin by using the difference in ' H spin-lattice relaxation time TlpHin the rotating frame for different hardwoods and softwoods [32]. Since the C1 and C6 resonance lines still seemed to contain unidentified contributions, the relative peak intensities of the most downfield and upfield lines of the C4 triplet were used to estimate the relative proportions of the I,, and I, forms. It was then concluded that the I,, fraction for softwoods was at almost the same level as for Vulonia-bacterialcelluloses,while the fractions for hardwoodsweresimilar to those for the cotton-ramie group. This conclusion may suggest that the crystallization of cellulose in woods will be affected in the presence of hemicelluloses and lignin, possibly resulting in the difference in fractions of I, and I, forms. A possible stress-induced crystallization of cellulose I,, which may be also induced in woods by the coexistence of hemicelluloses and lignin in the hybrid composites, will be described in the case of bacterial cellulose in a later section.
V.
CRYSTAL STRUCTURE OF CELLULOSES I, AND I,
As described above, the preliminary analysis of electron diffraction diagrams of celluloses I,, and I, were performed for delaminated fragments of Vulonia nzucrophysa. A more detailed microdiffraction analysis L331 was carried outalong single microfibrils with the widths of 25-35 nm that were separated from cell walls for Microdicryon, which is also a greenmarine alga. Two series of spot electron diffractogramswerealmostobtained independently, on different specimen areas with dimensions of about 50 nm, as shown in Figs. 10 and 1 1 . The diffraction spotsobserved in Fig. 10 are aligned in lines that are markedly inclined with respect to the cellulose chain axis (the long axisof the microfibril). I n all, 27independentreflections of this serieswereobtained, and all of themcanbe indexed using a one-chain P1 triclinic unit cell with cz = 0.674 nm, I? = 0.593 nm, c (chain axis) = 1.036 nm, a = 117", p = 1 I3', and y = 81'. This unit cell is found to be a singlechain version of the unit cell proposed by Sarko and Muggli [ 131. Another series of single-crystal diffraction diagramswereobserved for the same microfibrils, as shown in Fig. 1 I . In this case all the diffraction spotshaveorthogonal symmetry, indicating the monoclinic character. In fact, 38 independent diffraction spots observed in a l l as reflections of this series can be indexed in tcrms of a two-chain P2, unit cell with ( I = 0.801 nm, 0 = 0.817 n m , c (chain axis and unique monoclinic axis) = 1.036 nm. a = p = 90", and y = 97.3'. This unit cell is also found to be the same as unit cells [ 14,15,26,34-761 previously reported except for minor differences i n parameters ( I and y. The densities calculated for the triclinic and monoclinic unit cells are 1.582 and 1.599 g/cm', respectively. The significant increase in density for the monoclinic unit cell suggcsts the highcr thermodynamic stability of this unit cell compared to the triclinic unit
, -
8
. B
c
Ti4 0
@
O
110
O
FIGURE 10 A series of spot electron diffractograms presenting the triclinic features, which were obtained for the single microfibril of Microdictyon cellulose. (From Ref. 33, with permission of the American Chemical Society,Washington, DC.)
P 1
A
0 B
0
.
0
.
0
. . . 0
.
.
0
FIGURE 11 A series of spot electron diffractogramspresenting the monoclinic features, which were obtained for the single microfibril of Microdicryon cellulose. (From Ref. 33, with permission of the American Chemical Society, Washington, DC.)
I
-. P
Structure of Cellulose
95
cell, in good accord with the crystal transformation from cellulose I,, to I, as described above. Figure 12 shows the crystal structure models proposed for the one-chain triclinic and two-chain monoclinic phases on the basis of the microdiffraction analysis described above [33]. The monoclinic unit cell is the so-called Meyer-Misch-type cell, and the central chain in the cell is shifted downward by c/4 with respect to the comer chains. Moreover, this chain is rotated by 7.4” relative to the (200) plane, while there is no such rotation for the comer chains in the corresponding planes [33]. In contrast, when the central chain and the corner chains at the right side are shifted upward respectively by cl4 and 2d4 with respect to the corner chains at theleft side, one type of two-chaintriclinic unit cell can be obtained. Moreover, when the central chain is identical with the comer chains without any rotation with respect to the (200) plane, then another type of one-chain triclinic unit cell can be defined. This is the case for another allomorph of cellulose, cellulose I,, as shown in Fig. 12. As for the relative position of neighboring chains in the (1-10) plane of the one-chain triclinic unit cell, there are two possibilities, “parallel up” and“paralleldown.”Here, “up” or “down” indicates that the z coordinate of 0 5 is larger or smaller than the coordinate of C5, respectively. A molecular dynamic simulation in the crystalline environment was carried out by using the structure models of celluloses I, and I, shown in Fig. 12 as starting structures [37]. The program used was GROMOS 87 equipped with the appropriate force field. The triclinic phase was simulated under the periodic boundary condition for 4 X 6 X 3 (a X b X c ) unit cells with 2016 atoms, while the monoclinic phase was simulated for 3 X 3 X 3 unit cells with 15 12 atoms. It was found that the I, phase is energetically lower by 8.7 kJ mol-’ cellobiose-’ than the I, phase, in agreement with the almost complete crystal transformation from cellulose I,, to I, at higher temperatures [20,21]. Such higher stability in the I, form is due to intraplanar electrostatic interactions, particularly in the (200) plane. Moreover, the rotation of the chain in the (200) plane increases from 7.4” to I l S ” , resulting
Monoclinic Two-Chain Triclinic One-Chain
FIGURE 12 Crystal structure models of celluloses I, and I, assignable to the one-chain triclinic and two chain monoclinic crystals, respectively [33].
Horii
96
in significant changes in radial distribution functions and hydrogen bonding patterns, in addition to the reduction in energies. Structural features found for the triclinic and monoclinic phases were also qualitatively related to their spectroscopic features in FT-IR and CP/MAS "C NMR spectra. Similar molecular dynamics simulations were also performed using the CHARMM molecular modeling program, with the PARM 20 parameter set to characterize the differences in molecularmobilityandhydrogen-bondformation-breakage for the two allomorphs [38]. As a result of the simulation during 75 PS at 20°C after reaching the equilibrium state, it was found that the torsion angles 4 and IC, fluctuate with time on the order of 230" around the initial values for the I,, phase, whereas such fluctuations are only of the order of 10" for the I,. The time fluctuation of the chain center along the c axis was also considerably higher for the I, form than for the I, form. On the basis of these results, a break-slip model was proposed for the crystal transformation from cellulose I, to I,. In this model, it is suggested that the transformation is initiated by heat-induced torsional rotations of the CH,OH and OH groups accompanied by hydrogen-bond breakage. Cellulose chains are then subjected to rotation around the molecular chain axis and sliding along the axis, resulting in conversion to the I, form. For further reliable elucidation of the crystal structureforthesecelluloseallomorphs,however,parameters used in these simulations should be improved by comparison with experimental results.
VI.
CRYSTALLIZATION PROCESS OF NATIVE CELLULOSE
Even after the establishment of the composite crystal model for native cellulose, there still remains a question to be answered: how are celluloses I,, and I, crystallized in nature? The recent electron microdiffraction analysis described above also revealed that the I,, and I, phases are alternatively locatedwitha periodicity of about 100 nm along the single microfibril for Microdictyorz [33]. In the case of bacterial cellulose, such a periodic structure cannot be observed and almost one series of diffraction spots assignable to the I,, phase is obtained along the single microfibril [39,40]. Since the mass fraction of cellulose I, is 0.37, this phase must be located in the thin central core area along the microfibril, as will be described later. These facts suggest that the mode of distribution of the two allomorphs in single microfibrils may change from sample to sample and thus the crystallization of the allomorphs also depends on the conditions for the production of different cellulose samples.When the hemicellulosesand ligin coexistduring the crystallization process, effects of these materials should be well evaluated (411. In this situation, it will be very important to investigate the crystallization process in each system producing probably different composite crystals in nature. Here the case of the bacterial cellulose system is described in some detail, because this system has been considerablyinvestigated hitherto 142-441.
A.
Formation of the Normal Ribbon Assembly
It is well known that a gel-like pellicle of cellulose with a high water content is produced on the surface ofan incubation medium when a Gram-negative bacterium called AcetnDucter .ryylinum is cultured in anaqueousmediumcontainingacarbonsourcesuchas glucose at about 30°C. Such a macroscopic cellulose material is organized as a result of high-orderedaggregation of the normalribbonassemblies that are synthesized by the
Structure of Cellulose
97
FIGURE 13 Transmission electron micrographs of the negatively stained twisting ribbon assembly (a) and splayed microfibrils (b) produced in the presence of 1.0% CMC [19].
individual Acetobacter xylinum. Figure 13a shows a transmission electron micrograph of such a negatively stained normal ribbon assembly produced from a single bacterial cell. In Fig. 14 is shown schematically the process of the formation of the ribbon assembly from the bacterial cell on the basis of a large number of publications [42-441. More than several tens of cellulose-synthesizing sites are located in the cytoplasmic membrane, being parallel to the longitudinal cell axis. Cellulose synthetases in the respective sites produce 12-16 cellulose chains and extrude them into the culture medium as thin fibrils with a width of about 1.5 nm (often called subelementary fibrils) through small pores in the outer membrane. These subelementary fibrils aggregate with each other to form microfibrils, and the microfibrils furtheraggregate to produce the ribbon assembly with width 40-60 nm. The crystallization of cellulose will be induced during the different processesof the aggregations, because the subelementary fibrils may be too thin to be crystallized. In fact, subelementary fibrils have been confirmed to be noncrystalline for a specimen obtained by incubation in the presence of fluorescent brightening agents that prevent the aggregation of subelementary fibrils into microfibrils[42,43]. Since theparallel orientationof cellulose chains is already realized in the subelementary fibril, somewhat local-level rearrangements
Horii
98
shouldbeenoughtoinduce crystallization by aggregationinto the microfibril mainly through hydrogen bonding. Therefore, physicochemical factors affecting the aggregation process into microfibrils and the ribbon assembly will be associated with the crystallization of celluloses I, and I,. Of many possible factors, we first examined effects of the addition of different water-soluble polymers into the incubation medium on the formation of the two allomorphs, because carboxymethyl cellulose sodium salt and xyloglucan are known to interrupt the formation of the normal ribbon assembly [42-441. Low-molecular-weight compounds such as fluorescent brightening agents and direct dyes are also very effective in producing different types of fibrillar structures of cellulose. However, the crystallization into celluloses I, and I, is also highly interrupted in most cases [42-471.
B.
Effects of Polymeric Additives
Stationary cultures of Acerobacter xylinum were grown in Hestrin-Schramm’s medium at 28°C in the presence of carboxymethyl cellulose sodiumsalt (CMC), pea xyloglucan(XG), poly(viny1alcohol) (PVA), or poly(ethy1eneglycol) (PEG) [26,48]. Figure 15 shows CP/MAS I3C NMR spectra for bacterial celluloses cultured in the presence of the different polymeric additives [48]. The central line of the C l triplet decreases remarkably in intensity for bacterial celluloseincubated in the presence of 2.5 wt% CMC or 2 wt% XG, indicating the preferable crystallization of cellulose I, under such conditions. The increase in mass fraction of cellulose I, is also confirmed from the increase in intensity of the most upfield line in the C4 triplet and the concomitant decrease in intensity of the most downfield line. These changes were more clearly observed in the spectra of crystalline componentsrecorded selectively [48]. In contrast, almostnochange in relative intensity is observed in the C l and C4 triplets for the samples cultured in the presence of 20 wt% PVA or 25 wt% PEG. Similar addition effects were also reported for glucomannan as well as XG, and a marked decrease in crystallinity was found in the case of the former polysaccharide [49]. In Fig. 16 the mass fraction of cellulose I, is plotted against the concentration of CMC for samples with different degreesofpolymerization (DP) and different degrees of substitution (DS) [29]. Here, the mass fraction of the I, form was determined by the FT-IR methodbasedon Eq. (1). As is clearly seen in this figure, the mass fraction of cellulose I, decreases markedly with increasing CMC concentration. The most prominent decrease is observed for CMC with DP = 80 and DS = 0.57, suggesting the existence of an optimal DP and DS for the effect of CMC on the crystallization of the two allomorphs. Since there is almost no change in the degree of crystallinity in this system, CMC really promotes the preferable crystallization of cellulose I,, possibly as a result of the suppression of the crystallization of cellulose I,. Similar reduction in the mass fraction of the I, form was also confirmed in the case of XG, but the extent of the decrease was not so prominent even for the sample with the optimal molecular weight compared to the case of CMC [29]. As described above, CMC and XG interrupt the aggregation of microfibrils into the normal ribbon assembly, probably by the adsorption of CMC or XG on the surface of the microfibrils through hydrogen bonding. We have also confirmed such interruption of the aggregation by transmission electron microscopyasshown in Fig. 13bandfound that these splayed microfibrils were remarkably reduced in average diameter with increasing concentration of CMC or XG. Moreover, it has been finally clarified that there exists a simple linear correlationship with the mass fraction of cellulose I, and the average size of microfibrils for bacterial celluloses incubated in the presence of CMC, XG, and methyl
99
Structure of Cellulose
C
J
l
l
l
l
~
l
l
l
l
l
f
l
l
l
l
l
l
l
l
l
~
100
~
l
f
I
I
~
I
~
~
~
1
1
~
80
~
I
1
~
~
~
I
I
~
I
1
1
1
1
1
1
1
1
1
1
1
1
1
1
1
60 ppm f r o m T M S
FIGURE 15 CP/MAS "C NMR spectra for bacterial celluloses cultured in the presence of different polymeric additives: (a) control; (b) 2.0% XG; (c) 2.5% CMC; (d) 25% PVA; (e) 10% PEG [481.
[
1
1
1
1
l
*
~
Horii
100
1 0
0.5
1.o
1.5
Concentration of CMC l wt%
FIGURE 16 Mass fraction of cellulose I,, in bacterial cellulose cultured in the presence of CMC with various degrees of polymerization (DP) and degrees of substitution (DS) versus concentration of CMC: ( 0 ) control; ( 0 ) DP = 630, DS = 0.65; (A)DP = 80, DS = 0.57; ( 0 ) DP = 40, DS = 0.57; ( 0 ) DP = 80, DS = 1.43 [29].
cellulose [40,50]. It was therefore suggested that cellulose I,, is preferably crystallized in larger-size microfibrils, whereas cellulose I, is dominantly produced in thinner microfibrils. The mechanism of the preferential crystallization of celluloses I, and I, in microfibrils with different sizes will be discussed after the description of the crystallization of cellulose I1 in the bacterial cellulose system.
C.
Crystallization of Cellulose II in Nature
Cellulose 11, which is another representative crystal form of cellulose, is usually obtained by crystallization from a solution or by regeneration from alkali cellulose after mercerization. In the bacterial cellulose system the so-called native band material is sometimes observed in an irregular region where the normal ribbon assemblyisdisrupted by the formation of this material [42,44]. It has recently been revealed that such band material is composed of cellulose 11, by using a spontaneous variant of Acrtobucter xylinum that produces the band material as a main product under the standard culture condition [51,521. More recently, we have found that Acefobacter q l i n u m , which is collected from smooth colonies on a solidified Hestrin-Schramm medium, preferentially produces the native band material in incubationat 4"C, whereas the same bacterium produces the normal ribbon assembly at 28°C as usual [53].This indicates that the crystallization of cellulose I or I1 evidently depends on the culture temperature in this bacterial system. It is therefore very important to investigate this system in detail to clarify the mechanism of the crystallization
Structure of Cellulose
101
of celluloses I, and I, as well as cellulose II. Here, experimental results at the initial stage are briefly described, because investigation has just started with this system. Figure 17 shows transmission electron micrographs of the negatively stained band materialspreparedbyincubationfor 3 h in Hestrin-Schramm’s medium at 4°C on an electron microscope grid [53]. As is clearly observed in Fig. 17a, the band material is extruded out perpendicularly to the long axis. This band material seems to be composed of small irregular granules loosely linked to form strandlike structures in lying the direction of band extrusion, as pointed out in the previous paper [51]. However, when the micrograph is enlarged by 7.5 times as shown in Fig. 17b, most strands seem to be composed of irregularly coiled or folded thin fibrils. Since each strand is basically extruded from each pore on the surface of the bacterium in agreement with the previous finding [51], each strand will correspond to the subelementary fibril with an irregular coiled or folded appearance. In some areas parallel orientation of several units of the subelementary fibril are observed, but almost no discrete electron diffraction due to the crystalline entities could be detected for this band material by selected-area electron diffractometry. In contrast, three discrete diffractions are obtained on the equatorial line for the band material detached from the bacterium cell, as shown in Fig. 18 [53]. These three diffractions are well indexed as (1-10). (110), and (020) by using the unit cell of cellulose 11 [13], in good accord with the previous result [51]. Although they are considerably arced, molecular chain axes are confirmed to be almost perpendicular to the extrusion direction of the band bacterial. It is therefore concluded that cellulose 11 is partly formed in the native band material, but it is very important to obtain more informationabout the detailed structure of the band material, including the existence of folding structureof subelementary fibrils, which was suggested previously [51,52], to propose the mechanism of the crystallization of cellulose 11. In this bacterial system, another important finding is that the band material and the normalribbonassemblyaresequentiallyproducedwhentheincubationtemperatureis changed between 4°C and 28°C [53]. Figure 19 shows the drastic change in the cellulose production from the band material to the normal ribbon assembly as observed by electron microscopy. In this case a TEM grid with a culture drop containing Acetobacter xylinum that had been kept at 4°C for 5 h was transferred into an incubator regulated at 28°C and the culture was carried out there for 7 min. It is clearly found that the band material,
FIGURE 17 Transmission electron micrographs of the negatively stained native band material that was cultured at 4°C [53].
102
Horii
FIGURE 18 Selected-area electron diffraction pattern of the native band material detached from the bacterial cell. Three equatorial reflections are ascribed to those of (l-lo), (110). and (020) planes of cellulose II [53].
which was formed at 4"C, is linked sequentially to the normal ribbon assembly that is produced at 28°C. It is very difficult at present to describe how the production of the band material or the normal ribbon assembly is controlled in this system. However, the movement of the bacterium may be associated with the formation of these structures. Previous lightmicroscopic observation [42,44,54] revealed that the bacterial cell rotates around its longitudinal axis as it is propelled forward by the elongating ribbon during the production of the ribbon assembly. We also observed similar specific movements of the cells in the culture medium by a differential-interference light microscope with a TV system [55]. In
FIGURE 19 Sequential production of thenormalribbon assembly andthebandmaterial successive 28OC/4"C incubation of Acerobactor xylinum from the smooth colony [53].
by the
Structure of Cellulose
103
contrast, their movements are not specifically similar to the well-known irregular movements of Escherichia coli, when the cellulose is not produced. More careful observation of the movements of Acetohacter xylinum is necessary at 4 and 28°C to elucidate the processes of the different fibrillar structures.
D. Hypotheses on the Crystallization Mechanismof Celluloses I, and I, First it should be pointed out that the normal ribbon assembly shown in Fig. 13a is always twisted with a periodicity of about 1 p m around the longitudinal axis in one direction, possibly as a right-handed helix. Since such twisting is also observed for a long ribbon or intertwined ribbons, the twisting force must be induced not from the terminal of the ribbonbutfrom the cell sideduring or after the formation of the ribbonassembly. A previous report has suggested that the twist of the ribbon might be attributed to some property of cellulose molecules or to their interaction at the cell surface [43]. However, we can also see similar overall twisting for splayed microfibrils obtained by incubation in the presence of CMC, as shown in Fig. 13b. The latter type of twisting is not due to any cause attributed to the individual splayed microfibrils, particularly to cellulose molecules, but it could be produced simplyby the rotation of the bacterial cell around the longitudinal axis, which is usually observed by light microscopy as described above. It is therefore reasonable to assume that the overall rotation of Acefobacter xylinum also induces the twist of the normal ribbon assembly. During the production of the normal ribbon assembly the bacterial cell also moves translationally along the twisting ribbon axis together with the rotation. These cooperative movements will promote the aggregation of subelementary fibrils into microfibrils and furtherformation of the twisting ribbonassembly. In the incubation at 4"C, where the native band material is produced instead of the ribbon assembly, such specific movement may be hindered for some reason unknown at present, although subelementary fibrils are still allowed to be extruded into the culture medium. The next important problem is the possible effect of the rotational motion of the bacterial cell on the crystallization of celluloses I, and I,. Recently we have elucidated the effect of twisting a thin plate like the ribbon assembly. Figure 20 shows the process of twisting for a thin deformable plate PQRS around its longitudinal axis A. If the side PQ is rotated by angle 8 around the A axis under the fixation of the side SR, the longitudinal lengths PS and QR are extended to P'S and Q'R, respectively, by such twisting. When the plate is assumed to be deformed according to Hooke's law, the stress F produced by the twisting will be expressed as
Here, E is the Young's modulus of the plate along the longitudinal direction, r is the halfwidth of the plate, and 8 is the twisting angle around the A axis, which is defined for a given length L of the plate. Equation (2) clearly indicates that shear stress F, which is proportional to r2, is induced along the longitudinal direction of the plate, when the plate undergoes twisting around the long axis. The normal ribbon assembly is not a homogeneous thin plate as shown in Fig. 20, but the constituting microfibrils with somewhat different sizes are closely connected with each other, probably through hydrogen bonding. Moreover, the twist of the ribbon will be produced during the aggregation of the microfibrils. Nevertheless, when the normal ribbon assemblyundergoes twisting around the longitudinal axis before crystallization, shear
104
Horii
A P'
'
I
-r
FIGURE 20
-
Schematic diagram for twisting of a thin plate [19].
stress may be induced along the longitudinal axis in proportion to the squares of the half width of the ribbon. Under such shear stress, cellulose I,, will be preferentially produced through so-called stress-induced crystallization, because the orientation of the molecular chains in the I,, form seems to be organized by the shear stress along the chain axis. That is, the cellulose chains in a given ( 1 10) plane are shifted upward or downward by c/4 against the corresponding chains in the upward or downward successive (110) planes, as shown in Fig. 12. In addition, cellulose I, will be crystallized mainly in the regions along both edges of the ribbon assembly, because the shear stress is higher in those regions. In contrast, cellulose chains are packed in a more stable form in the unit cell for cellulose I,, asshown in Fig. 12. This type of crystal may beformedunder less shear stress or without shear stress, which may be referred to as stress-jree crystcrllization. According to the structural model shown in Fig. 20, cellulose 1, will be crystallized in the central core region because the shear stress is less or free in this region. When the ribbon assembly is partly disordered or splayed into somewhat thinner microfibrils, such a part may be also composed of cellulose 1, because the twisting induces much less shear stress for disordered or smaller-size microfibrils. The dependence of the mass fraction of cellulose I, on the size of microfibrils described in the previous section is also well interpreted in terms of the structural model shown in Fig. 20. In the case of Microdicfyon cellulose, in which 1, and I, crystals appear alternately along a single microfibril as describedabove [331, another crystallization mechanism should be proposed: the so-called two-step orientationcrystallization [ 191. Before the initialization of the crystallization, the cellulose chains are highly oriented in each microfibril just as in the liquid crystalline state, but they are not fully extended to the molecular chain length. Therefore, after the crystallization of cellulose I,, under some different stress (stress-induced ctystallization), the residual part of such chains left in the noncrystalline state will be relaxed in length as a result of the full extension of the crystalline chains. This willlead to the relaxation of the stress, andthen anothertype of crystallization,
Structure of Cellulose
105
stress-free crystallization, may occur to form cellulose I, in the central part of the noncrystalline region. Thissuccessivetwo-step orientation crystallization will producethe alternate I, and I, crystals along the single microfibril. Finally, it should be noted that cellulose I can be crystallized in vitro after a cellulasecatalyzedpolymerizationofP-cellobiosyl fluoride substratemonomer in acetonitrile/ acetate buffer [56].Under the normal condition employing unpurified cellulases, cellulose I1 is crystallized in a reaction medium after the polymerization as expected in analogy of the crystallization of cellulose from the solution [57]. In contrast to this fact, the cellulose I allomorph was confirmed by selected-area electron diffractometry for fibrous materials produced by using substantially purified cellulaseenzyme,although the discrimination between the I, and I, forms was not achieved [56].Such an interesting result may be due to the parallel orientation of extended cellulose chains with the same polarity, which is assumedto be organized as a result of a micellaraggregation of the partially purified enzyme and the substrate in the nonaqueous/aqueous solvent system. More detailed investigations of this system will also contribute to the exact interpretation of the crystallization mechanism of native cellulose.
VII. CONCLUDINGREMARKS As described above, the composite crystal model has been established in native cellulose, although there may be minor exceptions depending on the sources of cellulose. Nevertheless, the detailed structure, such as the chain conformation, hydrogen bonding, and molecular packing, has not yet been clarified in both allomorphs because precise structural analyses of the intensities of X-ray or electron diffraction diagrams have not been performed systematically so far. The situation is more serious for cellulose I,, because no pure I, specimen is available yet either in nature or by an artificial method. As a better way, the analysis will be made for specimens with higher contentsof the I,, form, assuming the linear combination of diffraction intensities of the I, and I, forms. In that case it should be taken account that the I, form is frequently subjected to some modification depending on the source of cellulose as shown in Fig. 3. As for the crystallization processes of celluloses I, and I, as well as cellulose I1 in nature, more detailed observations are necessary for the microfibril or subelementary microfibril structure at the level of several nanometers to several tens of nanometers by transmissionelectronmicroscopyandalso for the overall movementsof Acerobacter xylinurn by high-performance light microscopy. Information about the enzymatic degradation, acid hydrolysis, alkaline treatments, etc., for microfibrils, which is not described here because of space limitations, will be also very helpful for understanding the structures of microfibrils andsubelementary microfibrils. Through these investigations ourunderstanding of the structure of native cellulose will be greatly advanced in the next 5 or 10 years.
ACKNOWLEDGMENTS
The author thanks Dr. Asako Hirai and Hiroyuki Yamamoto for their constant cooperation throughout the work described here. He is also grateful to Prof. Masaki Tsuji and Prof. Junji Sugiyama for their kind cooperative contributions to structural analyses by electron microscopy.
106
Horii
REFERENCES 1 . S. Nishikawaand S. Ono, Proc. Tokyo Math.-Phys. Soc., 7131 (1913). 2. K. Okamura, in Wood and Cellulosic Chemistry (D. N.-S. Hon and N . Shiraishi, eds.), Marcel Dekker, New York and Basel, p. 89 (1991). 3. L. M. J. Kroon-Batenburg, and J. Kroon, Carbohydrate in Europe, p. 15 (1994). 4. A.C.O’Sullivan, Cellulose, 4: 173 (1997). 5 . R. H. Atalla, J. C. Cast, D. W. Sindorf, V. J . Bartuska, and G. E. Maciel, J . Ant.Chern. Soc., 102:3249 (1980). 6. W. L. Earland D. L. VanderHart, J. Am. Chem. Soc., /02:3251 (1980). 7. F. Horii, A. Hirai, and R. Kitamaru, Macromolecules, 20:2117 (1987). 8. F. Horii, in Nuclear Magnetic Resonance in Agriculture (Pfeffer, P. E., Gerasimowicz, W. V., eds.), CRC Press, Boca Raton, FL, chap. 10 (1989). 9. F. Horii, A. Hirai, and R. Kitamaru, J. Carbohydr.Chem., 3:641 (1984). 10. A. Hirai, F. Horii,andR.Kitamaru, CelluloseChem.Technol., 24:703 (1990). 11. H. J. Marrinan and J. Mann, J. PolymerSci., XXI:301 (1956). 12. G. Honjo and M.Watanabe, Macromolecules, /81:326 (1958). 13. A. Sarko and R. Muggi, Macromolecules, 7486 (1974). 14. K. H. Gardnerand J. Blackwell, Biopolymers, 13:1975(1974). 15. C. Woodcock and A. Sarko, Macromolecules, 13:1183(1980). 16. R. H. Atalla and D. L. VanderHart, Science. 223:283 (1984). 17. D. L. VanderHart andR. H. Atalla, Macromolecules, /7:1465 (1984). 18. H. Yamamoto and F. Horii, Macromolecules, 26: 13 13 ( 1993). 19. F. Horii, H. Yamamoto, and A. Hirai, Mucromol. Symp., 20: l97 (1997). 20. F. Horii, H. Yamamoto, R. Kitarnaru, M. Tanahashi, and T. Higuchi, Macron~olecules,20:2946 (1987). 21. H. Yamamoto, F. Horii, and H. Odani, Macromolecules, 22:4130 (1989). 22. A. Hirai, F. Horii, and R . Kitamaru, Macromolecules, 20:1440(1987). 23. H. Chanzy, B. Henrissat, M. Vincendon, S. F. Tanner, and P. S. Belton, Cnrbohydr. Res., 160: 1 (1987). 24. M. Tanahashi, T. Goto, F. Horii, A. Hirai, and T. Higuchi, Mokuzai Gakkaishi, 35:654 (1989). 25. E. M.Debzi, H. Chanzy, J. Sugiyama, P. Tekely, and G. Excoffier, Macromolecules, 246816 (1991). 26. J. Sugiyama, T. Okano, H. Yamamoto, and F. Horii, Macromolecules, 23:3196 (1990). 27. J. Sugiyama, J. Persson, and H. Chanzy, Macromolecules, 24:2461(1991). 28. J. H.Wiley and R. H. Atalla, in The Structure of Cellulose (R. H. Atalla, ed.), ACS Symp. Ser. 340, American Chemical Society, Washington, DC, p. 151 (1987). 29. H. Yamamoto, F. Horii, and A.Hirai, Cellulose, 3:229 (1996). 30. P. S. Beleon, S. F. Tanner, N. Cartier, and H. Chanzy, Macromolecules, 22:1615 (1989). 31. M.Wada, T. Okano, J. Sugiyama, and F. Horii, Cellulose, 2:223 (1995). 32. R.H.Newman, J . WoodChem.Technol., 14:451(1994). 33. J. Sugiyama, R. Vuong, and H. Chanzy, Macromolecules, 24:4168 (1991). 34. K. H. Meyerand L. Misch, Helv. Chim. Acta, 11534 (1937). 35. D. P. Miller and A. Li, in Cellulose and Wood, Chemistty and Technology (C. Schuerch, ed.), Wiley, New York, p. 139 (1989). 36. R. P. Millaneand T. V. Narasaiah, CelluloseandWood:Chetnistty und Technology (C. Schuerch, ed.), Wiley, New York, p. 39 (1989). 37. A. P. Heiner, J. Sugiyama, and 0. Teleman, Curbohydr. Res., 273:207 (1995). 38. B. J. Hardy, and A. Sarko, Polymer; 37:1833(1996). 39. F. Horii, A. Hirai, H. Yamamoto, and J. Sugiyama, Preprinfs of the3rdAnnual Meeting of the Cellulose Society of Japan, published by the Cellulose Society of Japan (% Institute for Chemical Research, Kyoto University), p. 1 1 (1996). 40. A. Hirai, F. Horii, M. Tsuji, J . Sugiyama, and H. Yamamoto, Proc. 1st Int. Symp. Inst.Chem. Res., Kyoto Univ. (ICRIS ’96), p. 132 ( 1 996).
Structure of Cellulose
107
41. Y. Kataoka and T. Kondo, Macromolecules, 29:6356 (1996). 42. C. H. Haigler and M. Benziman, in Cellulose and OtherNatural Polymer Systems. Biogenesis, Structure and Degradation (R. M. Brown, Jr., ed.), Plenum Press, New York-London, p. 273 (1982). 43. C. H. Haigler and H. Chanzy, in Cellulose and Wood: Chemistry andTechnology (C. Schuerch, ed.), Wiley, New York, p. 493 (1989). 44. C. H. Haigler, inBiosynthesis and Biodegradation of Cellulose (C. H. Haigler and P.J. Weimer, eds.), Marcel Dekker, New York-Basel-Hong Kong, p. 99 (1991). 45. A. Kai and H. Kitamura, Bull. Chem. Soc. Japan, 58:286 (1985). 46. A. Kai, F. Horii, and A. Hirai, Mucromol. Chem., Rapid Commun., 12:15 (1991). 47. A. Kai, P. Xu, F. Horii, and S. Hu, Polymer; 35:75 (1994). 48. H. Yamamoto and F. Horii, Cellulose, 1:57 (1994). 49. J. M. Hackney, R. H. Atalla, and D. L. VanderHart, Int. Bio. Mucromol., 16:215 (1994). 50. A. Hirai, H. Yamamoto, M. Tsuji, and F. Horii, Proc. '94 Cellulose R&D, Cellulose Society of Japan, p. 41 (1994). 51. S. Kuga, S. Takagi, and R. M. Brown, Jr., Polymer; 34:3293 (1993). 52. H. Sibazaki, S. Kuga, F. Onabe, and R. M. Brown., Jr., Polymer; 36:4971 (1995). 53. A. Hirai, M. Tsuji, and F. Horii, Cellulose, 4:239 (1997); more detailed results will be published elsewhere. 54. R. M. Brown, Jr., and D. Montezinos, Proc. Natl. Acad. Sci. USA, 73:143 (1976). 55. A. Hirai and F. Horii, to be published. 56. J. H. Lee, R. M. Brown, Jr., S. Kuga, S. Shoda, and S. Kobayashi, Proc. Natl. Acad. Sci. USA, 91:7425 (1994). 57. S. Kobayashi, K. Kashiwa, T. Kawasaki, and S. Shoda, J. Am. Chem. Soc., 113:3079 (1991).
This Page Intentionally Left Blank
Chemistry of Lignin Akira Sakakibara and Yoshihiro Sano Hokkaido University, Sapporo, lapan
1.
INTRODUCTION
Lignin exists as one of the essential wood components, ranging in amount from 10% to 30%. It is thought that lignin is a polymer formed by the enzymatic dehydrogenation of phenylpropanesfollowed by radical coupling.Softwood lignin is composedmainly of guaiacyl units originating from the predominant precursor, rrans-coniferyl alcohol (l), while hardwood lignin is composed of both guaiacyl andsyringyl units derived from transconiferyl (L) and trans-sinapyl (2) alcohols, respectively. Grass lignin contains p-hydroxyphenyl units derived from trans-p-coumaryl alcohol (3),besides units originating from the foregoing two precursors. However, strictly speaking, almost all plants consist more or less of all three units, namely, guaiacyl, syringyl, and p-hydroxyphenyl moieties. Lignin has no optical activity, in contrast to other compounds, because the radicals formed by enzymatic dehydrogenation couple with one another at random to give the lignin polymer. (OH
OH
(OH
OH
con OH
Lignin is the mostcomplexpolymeramong naturally occurringhigh-molecularweight materials, and investigations devoted to the elucidation of its structure have been under way for a long period of time. The presence ofmany complex carbon-to-carbon linkages between the units makes it difficult to degrade the polymer to low-molecularweight fragments. Furthermore,it has not yet been possible to isolate all parts of the lignin completely from plant tissues without engendering structural changes. [Bjorkman prepared milled wood lignin (MWL) that hasundergone little change,butalthough it is a very useful preparation, the yields are at most 50% of Klason lignin.] These characteristics make it hard to elucidate the chemical structure of lignin. The biosynthesis of lignin in vitro, worked out by Freudenberg and co-workers, provided guidance in approaching this 109
110 San0
and
Sakakibara
problem. Information on the degradation products from protolignin could provide direct evidence about lignin structure. For this purpose, the following procedures for bringing about lignin degradation are effective: catalytic hydrogenolysis, controlled hydrolysis, and degradation by thioacetolysis or thiacidolysis followed by reduction. As complementary procedures, oxidations of lignin with KMnO,, nitrobenzene under alkaline conditions, and acidolysis are available. The quantitative data for various functional groups and linkage types in protolignins are also essential to understanding lignin structure. Ultraviolet (UV), infrared (IR), and nuclear magnetic resonance (NMR) spectroscopic techniques, particularly when used in conjunction with chemical modification, have contributed to estimating the frequencies of functional groups and linkage types. Some lignin structural models could be proposed from these combined studies, but they do not represent a strict molecular structure such as those for other natural polymers such as cellulose and proteins. This may be unavoidable, however, in view of the biogenetic mechanism governing the formation of lignin.
II. SPECTROSCOPY
A.
Ultraviolet(UV)Spectra
Ligninshows a strongabsorptionspectrum in the UV region, becauseof its aromatic nature. The lignin spectrum of a typical softwood in Fig. 1 [ l ] has two maxima at 205 and 280 nm, shoulders at 230 and 330 to 340 nm, and a minimum at 260 nm. In general, softwood lignin shows a maximum at 280 to 285 nm, and hardwood lignin at 274 to 276 nm [ l ] . As the method is verysimple, UV spectrophotometric investigations are used extensively to characterize lignin preparations. Aulin-Erdtman [2-51 applied UV spectra to estimate effectively the amounts of certain functional groups, especially the phenolic hydroxyls of lignin, by means of differ-
200
250
300
350
400
450 nm
FIGURE 1 UV spectra of pine and beech lignins and
A E curve for pine lignin. (From Ref.
1.)
Chemistry of Lignin
111
entia1 measurements.Both the ionizedhydroxylandaldehydegroupscauseamarked bathochromic spectral shift. The phenolic hydroxyl content in polymers can be determined by comparing the adsorptionspectra in neutral andalkalinesolutions.Understrongly alkaline conditions, the absorptivity in the wavelength region of maximum adsorption for the phenolate ion is increased. The magnitude of this increase can be used quantitatively to determine the amount of phenolic hydroxyl groups. With this A&, method, Aulin-Erdtman [2]estimated the phenolicgroupcontentforsolublederivativesofspruce lignin (Picea abies) andBrauns’ lignin (BL) from Piceamariana and Tsugaheterophylla, in addition to DHP (a synthetic dehydrogenation polymer) by comparison with appropriate models. Further, phenylcoumaran and coniferyl aldehyde structures could be characterized spectrophotometrically [3].More closely related model compounds, such as coniferyl (L), sinapyl and dehydrodiconiferyl (M)alcohols, were also investigated with this A&, method [4]. From studies of about 40 p-substituted compounds, a series of regular absorptiondifferenceswerefoundbetweenthem [ 5 ] . A marked effect fromo-methoxyl groups on the planarity of 2,2-dihydroxy-biphenyls was observed. Biphenyl compounds showed a higher degree of coplanarity in dioxane, in which hydrogen bonds exist between the phenolic hydroxyls and solvent. The mono-ol showed a smaller interplanar angle in hexane, due to the presence of a seven-membered 0-H-O-H-OCH3 “ring” than in an acidic dioxane solution. where OH-dioxane bonds dominate.
(z),
(I)
OH
OH W
0 ,
.bCH3
H“
Pew [6] found that C-4-substituted guaiacyl and related compounds with unconjugatedsidechainsshow similar andalmost identical curves, as shown in Fig. 2 . These model compounds haveultraviolet absorption maxima at 280 nm, but unlike that for lignin, the curve tills abruptly to zero at 300 nm and nearly to zero at 250 nm. The filling in of the spectral trough at 250 nm in lignin can be explained by the presence of biphenyllinked units (Fig.2). Until then, biphenyl units in lignin molecules had generallybeen assumed to be minor contributors, butPew [7 I presumed that coniferous lignin may contain considerable biphenyl-linked units. A simpleand rapid method for the determination of phenolichydroxylgroups in lignin preparations was developed by Goldschmid [8] based on the A&, method. The phenol content of the sample is calculated from the absorptivity maximum of the resulting difference curve, and the molar absorptivity maximum of model phenols is determined i n the samemanner. The 300-nm maximum of the differencecurves is characteristic of phenolic hydroxyl groups without con.jugation. The method is suitable for routine appli-
112
Sakakibara and San0
1.0
0.8
E 0.6 m
-2 S1
2
0.4
0.2
0
300 320340360400
230240250260270280290
A-mp
FIGURE 2 UV spectra of spruce cellulytic enzyme lignin and of C4substituted unconjugated guaiacyl compounds. (From Ref. 6.) cation to technical softwood lignin preparations. Phenylcoumaran (g) (Arna 281 nm) undergoes dehydration during acidolysis to give a phenylcoumarone structure which has a strong absorption band at maximum 310 nm. By studying the spectral curves of these compounds, Adlerand Lundquist [9] estimated the contentof phenylcoumaran units in lignin. Schdning and Johansson [lo] studied the W absorption of lignin from pulp waste liquor and concluded that acid-soluble lignin components should be determined at 205 nm, because the absorption maximum at 280 nm is influenced by degradation products from carbohydrates, such as furfural. It was found that wood samples from spruce and pine contain 0.2%acid-soluble lignin, from birch and eucalyptus 3-4%, from wheat straw 2%, and from bamboo 1.5%. Klason lignins, especially those from hardwood, must be corrected for the acid-soluble lignin content. Wegener et al. [l11 found that hexafluoropropanol is an excellent solvent for UV and IR spectroscopy of lignins, because the absorption maximum of water-insoluble samples near 200 nm can be recorded exactly and evaluated quantitatively, due to the high UV transmittanceproperties of thissolventwithoutinterferencefromthedegradation products of polysaccharides.
(B),
B.
Infrared(IR) Spectra
Infrared (R) spectroscopy has been used often for the characterization of lignin because the technique is simpleand the sample to be studied does not need to be dissolved in any solvents and is required only in very small quantity. Qpical IR spectra of soft- and hardwoods are shown in Fig. 3. Various lignin preparations can be easily compared using this technique. Assignment of various absorption bands of lignins in IR spectra has been stud-
113
Chemistry of Lignin
I
I so0
I
I
I
1
I
1600
1100
120c
1000
800
Wavenurnber (cm")
FIGURE 3 FTIR spectra of MWLs from oak, birch, and spruce. Legend: oak (Q~erc-uscrispcln Blurne), birch (Berrrla plntyphylln Sukatchev var. jcrponicn Hara), and spruce (Pinus glehnii Mast.).
ied by a number of lignin investigators, using a variety of methods. The major absorption band frequencies and the most probable assignment of each band in guaiacyl and guaiacylsyringyl lignins are shown in Table I , which has been somewhat supplemented from that summarized by Hergert 1 1 21. Kolboe and Ellefsen [l31 used IR spectroscopy as an independent method for estimating lignin content and coumaran groups. The absorption at 1515 cm" was chosen for the determination of lignin, because this region is assigned to aromatic skeletal vibrations. The lignin content was estimated by the difference spectrum between the original wood and holocellulose at ISIS cm-', giving 28-29%. Thatis in agreement with the value generally accepted. Further, the absorption band at 1495 cm" was assigned to the coutnaran ring, and it was estimated to contribute about 5% of the total phenylpropane units. Sarkanen et al. 1141 comparcd the spectra of specifically deuterated guaiacyl and syringyl models with thosc of undeuterated lignin models, to give several new band assignments. From these deuteration studies, the hitherto unidentified bands at 1450 to 1420 cm" were considered to be associated with the ring-stretching modes strongly coupled with the CH in-plane deformation similar to the l SO0 c m - ' band. The 1340- l380 and 1250- l l SO cm" bandswere usually assigned to phenolic hydroxyl groups. The latter 1250- I 150 cm I band may be described as an "0-H in-plane deformation with ring-stretching character," and the 1340- 1380 cm ' band a s having a "ring-stretching with 0 - H bending character." The 1240 cm ' band scctncd to have the most pronounced methoxyl character,
and
114
Sakakibara
San0
TABLE 1 Assignment of Infrared Absorption Bands in Mildly Prepared Wood Lignins Band (cm"')"
Hardwood
2880
1595 1505
Softwood lignin
3450-3400 3425-3400 2940 2920 2875-2850 2820 1715-1710 1715 1675-1660 1650-1630 sh 1605 1515-1510 1495 1470- 1460 1430 1370 1270 1230 1 l40
970 915 860
Assignment stretching0-H C-H
1470- 1460 1425 1370- 1365 1330- 1325 1235-1230 1275
1085 1035
1030
970 855 815 750-770 sh
Carbonyl stretching in unconjugated and ketone conjugated carboxylic groups Carbonyl stretching in conjugated ketone groups Carbonyl stretching in y-lactone skeletalAromatic vibrations
1675-1660
1145 1130 1085
stretching methylene ingroups and methyl
Coumaran ring C-H deformations (asymmetric) Aromatic skeletal vibrations C-H deformations (symmetric) Syringyl ring breathing with C-0 stretching Guaiacyl ring breathing with C-0 stretching
C-H inplane deformation in guaiacyl C-H inplane deformation in syringyl C-0 deformation in secondary alcohol and aliphatic ether C-H in-plane deformation in C-0 guaiacyl, and deformation in primary alcohol (trans) deformation out-of-plane =CH Aromatic C-H out-of-plane deformation sh
750 sh
"sh: shoulder. Source: Ref. 12.
because on methylation, the intensity of the 1240 cm" band increases at the expense of the 1275 cm" band. MWLs from the sapwood of several wood species have been characterized by analytical and spectral methods [15]. The results indicate that the basic lignin structure of conifers is almost the same, and the differences between wood species seem to be the differences in the identity and amount of ester groups ( l 7 15 cm- ') related to various lignins. The IR spectra of lignins isolated from whole wood samples that include heartwoodshowedan extra absorptionband at 1630 cm", whichwas totally absent in the MWL from sapwood. Also, the IR spectrum of larch lignin showed a weak peak from a conjugated carbonyl group at 1670 cm-'. These extra bandsthat may originate from polyphenols were considered to be indicative of the chemical modification of lignin during the heartwood formation process. It was also demonstrated that the infrared spectrum is useful
Chemistry of Lignin
115
asan indicator of the ratio of syringylpropane to guaiacylpropane units in heartwood lignins [ 161.
C.
Nuclear Magnetic Resonance (NMR) Spectra
The magnetic resonance spectrophotometric technique is very useful to lignin chemistry, because it gives a variety of information on the lignin molecule that cannot be obtained by ordinary chemical analysis. Especially as quantitative data about linkage types obtained by chemical methods are incomplete, this technique will supplement such deficiencies.
1. Proton Magnetic Resonance (‘H NMR) Spectra Ludwig et al. [ 17,181 were the first to obtain ’H NMR spectra of lignin and its model compounds,usingdeuterochloroformasasolvent(Fig. 4). The chemical shifts of the NMR signals from protons in various model compounds, including biphenyls, p-0-4 dilignols phenylcoumarans (E),and pinoresinol (g), were determined. The NMR of dehydrodiconiferyl alcohol indicated a cis configuration in its furan ring, and the diequatorial configuration of pinoresinol (g) was confirmed. Thereafter, the NMR spectra of acetylated dioxane lignin, MWL, and BL were interpreted using the results from lignin model compounds [18]. It was found that semiquantitative estimates on the free benzylic hydroxyls, aliphatic and aromatic hydroxyls, and total aliphatic hydrogens in the lignin preparationswere possible. Moreover, it wasfound that NMRspectroscopy affords a unique method for estimating the degrees of condensation in lignin preparations.
(z),
(m)
0
0
f ;
1
A HCCl3
HMD
I
8.48 7.81 7.50 5.18 5.74 6.28
8 FIGURE4 Ref. 18.)
7
9.95
4
5
6
7
8
9
10
6
‘H NMR spectrum of acetylated spruce MWL (60 MHz, solvent: chloroform-d). (From
116 San0
and
Sakakibara
The presence of highly shielded protons in the range 6 1 SS-0.38 is noticeable. These protons are clearly due to methyl or methylene groups that are not attached directly to oxygen functions, carbonylgroups,aromaticsystems,orotherdeshieldinggroups,but their structural origin seems to be hydrocarbon contaminant because lignin does not include these groups. Lenz [l91 studied ‘H NMR spectra of bothunderivatizedandacetylated lignins, using various deuterated solvents. Twelve lignin preparations, including MWL, kraft and soda lignins, and dioxane lignin, were examined. It was found that alkali and acidolysis lignin preparations from both hard- and softwoods showed marked differences in the degree of condensation of aromatic rings, phenolic and aliphatic hydroxyl groups, and the number of highly shielded aliphatic protons. Spruce MWL gave a proton distribution close to that found by Ludwig [IS]. Bland and Sternhell [20] obtained from ‘H NMR spectra estimates of the fraction of protons attached directly to aromatic nuclei in some lignin preparations from Pinus radiata and Eucalyptus regnans. They estimated the frequencies of “condensed” units in the lignin molecule; those in methanol and acetylated lignin from E. regnans and methanol lignin from l? radiata are 0.60, 0.66, and 0.71/OCH3, respectively. However, it should be noted that the condensed units here are aromatic rings in which at least one carbon atom, not necessarily the 5-carbon alone, is linked directly to another carbon atom outside the ring. According to Morohoshi et al. [21], NMR spectra indicate that the degrees of condensed units in lignins from normal wood and compression wood of Abies sachalinensis are 0.48 and 0.79, respectively. Also,from the results of the other analytical data, the structure of compression wood lignin is generally composed of more condensed units. Horisaki et al. [22] estimated the frequencies of “condensed units” in lignins using methoxyl content, the ratio of guaiacyl and syringyl rings, and proton numbers assigned to aromatic rings, ethylene groups, and benzyl alcohol groups obtained by the NMR (500 MHz) of acetylated lignins and their hydrogenation derivative-containing internal standard (p-nitrobenzaldehyde) for quantitative analysis. They foundthat the contents of condensed units and benzyl alcohol groups are 0.35 and 0.29/CCJin spruce MWL, and 0.30 and 0.451 C, in birch MWL. The formylprotons in the lignin moleculecould not bedetectedwithlower-frequency (60-MHz) NMR spectrometers [ 17-19]. Later, Lundquist and Olsson [23] studied the formyl groups in spruce lignin at 270 MHz and found that the signals in the range 6 9.6- 10.0 were essentially due to the protons of aldehyde and vanillin units. By integration, the amount of coniferyl aldehyde units was determined to be 4%. MWLs from birch 1241 and spruce [25] were further studied. The spectra are shown in Fig. 5. The use of a 270MHz instrument and new techniques have greatly increased the amount of available structural information. Signals in the spectra of acetylated birch and spruce lignins are summarized in Table 2. The peak at 6 308 of birch lignin was attributed to H,, in p-p structures, and integration suggests that around 0.05/C,,C3 are involved in @-pstructures. The peak at 6 5.44 was assigned to H in p-5 structures or noncyclic benzyl aryl ethers, and 6 4.60 (H,) and 6.01 (HJ were essentially attributed to p-0-4 structures. Integration of the 6.01 peaksuggested that 40-50% of the units are attached to an adjacent unit by a p-0-4 linkage. In the case of spruce MWL, the peak at 6 2.28 (aromatic acetate) was found to correspond to 0.26 phenolic groups/C,J (although certain phenol groups in biphenyl structures are not included in this estimate [ 17,181. From the peak at a 6 2.62 attributed to H,, in p-p structures, 0.01 to 0.02/C,C, were estimated for dihydrofuran or open-type p-p units. Later, however,from the results of studies usingdeuterioacetonesolutions [261, higher values of 0.02 to 0.03/C,C3 were obtained. The integral of the 6 5.49 peak, H,, i n
Chemistry of Lignin
117
FIGURE 5 Spectral range 6 8.0- 10.5 (400 MHz, solvent DMSO-d,) of MWL from spruce. Notes: the assignments of the peaks are indicated in the figure (the peak at 6 8.14 is due to an identified contaminant). The dashed lines indicate the baselines used in the connection with quantitative estimates. (From Ref. 27.)
p-5 structures, corresponds to about 0.1 l/C,C,. p - 0 - 4 substructures were estimated to be 0.3 to O.5/C,C3 by integration of the 6.06 (H,) peak from p-0-4units. Li andLundquist[27]studiedphenolicgroups in ligninsanalyzed by the NMR spectrometry at 400 and 500 MHz using DMSO-d, and 300 K as shown in Fig. 6. Under the conditions the majority of the signals from protons in phenolic hydroxyl groups are found at 6 8.0-9.3, and those in most carbonyl-conjugated phenols at >9.3. They estimated that the number of phenolic groups in spruce MWL is 0.24/C9, of which about20% originatefromphenolicgroups (6 8.1 -8.4) in biphenyl and diary1 ethersubstructures. Spectra of MWL from birch exhibited separate peaks for phenols in guaiacyl units (6 8.59.1) and syringyl units (6 8.1-8.2), though the latter peaks overlap with those for biphenyl substructures. The total number of phenolic groups was estimated as 0.18/C,, in which the proportion in guaiacyl and syringyl units is 3:2. Ede et al. [28] studied 'H-'H COSY and J-resolved spectra of acetylated MWL from spruce,concluding that the results confirm thepresence of most of the known lignin structural units, but show a-0-4 aryl ether, p - l , and @-punits to be less significant in lignin structures than were previously thought because of no existence of each cross-peak.
2. Carbon-l3 Magnetic Resonance (I3CNMR) Spectra Ltidemann and Nimz [29-311 were the first tostudy "C NMR spectra of lignins. The chemical shifts of various carbons in lignin model compounds were assigned, and also the effect on the chemical shifts of the aromatic carbon atoms from methoxyls ortho to the 4-phenolic hydroxyl group was studied [29]. When a methoxyl group is introduced into an aromatic ring, the substituted carbon shifts about 32 ppm to a lower field, but on the other hand, both the ortho- and para-carbon atoms shift to a higher field.
118
Sakakibara and San0
TABLE 2 Assignments of Signals in the 'H NMR Spectra of Acetylated Birch and Spruce MWLs in Chloroform-d
S unitslppm 1.26 2.01, 1.95, 2.02 2.13 2.28-2.29 2.94 3.08 3.76-3.8 I 4.18, 4.27-4.28 4.39 4.43 4.60 4.65 4.70 5.44 5.49 6.0 1-6.06 6.93-6.94 7.4 1 7.50 7.53 9.64 9.84-9.86
contaminantHydrocarbon Aliphatic acetate Aliphatic acetate (including aromatic acetate in biphenyl structure) acetate Aromatic Unknown absent peak (the is in acetate the of lignin reduced with NaBH,) Hp in p-p structures Protons in methoxyl groups H, in several structures H, primarily in p - 0 - 4 (erythro) and p-5 structures H,structures in several H, in p - 0 - 4 structures (birch) H,, in p - 0 - 4 structures (spruce) including methylene protons in cinnamyl alcohol units H, in p-p structures (birch) including methylene protons in cinnamyl alcohol units H, in p-5 structures noncyclic and benzyl ethers aryl (birch) H,, in p-5 structures noncyclic and benzyl aryl ethers and H,, in aryloxypropiophenones (spruce) H,, in p - 0 - 4 and p-l structures, and vinyl protons Aromatic and vinyl protons Aromatic protons in benzaldehyde units, vinyl protons carbon the on atom adjacent to aromatic rings in cinnamaldehyde units (spruce) Aromatic protons located ortho to carbonyl groups (birch) Aromatic carbonyl protons groups located (spruce) to ortho protons Formyl in cinnamaldehyde units Formyl protons in benzaldehyde units
On the basis of the model compounds, the various signals of the "C NMR spectra of beech and spruce MWLs were assigned [29]. The spectra of DHP, spruce and beech ligninsareshown in Figs. 7 and 8, respectively. The numbering 1-40 of the peaksis convenient for comparing these spectra. The assignment o f . these carbon atoms is summarized in Table 3. These chemicalshiftscan be divided roughly intothreereg' 'Ions: carbonylcarbonsappearat 6 200- 160 (with respect t o TMS as a standard), Cl -C6 aromatic carbons, C,, and C, of double bonds on the side chain, at 6 160- 1 0 0 , and other saturated side chains C,,, C,,, and C, at 6 90 to 20. Methoxyl carbons always appear in the narrow range of 6 56.3 t 0.2. From these peak assignments, it was concluded that the content of phenylcoumaran units i n spruce lignin is much more than that in beech lignin and presumed that the content of dioxabicyclo-octane units [pinoresinol (3) and/ or syringaresinol (g)] of beech lignin may be more than that of sprucc lignin. The "C NMRspectra of thedehydrogenationpolymers."Zulauf"-and"Zutropf"-DHPs.were compared with thosc o f sprucelignin 1301, indicating that the conditions of formation
119
Chemistry of Lignin
I
6
9
8
7
6
5
4
3
I
I
2
1
0
FIGURE 6 ' H NMR spectra (270 MHz) of acetylated MWLs from birch and spruce wood. (From Refs. 24 and 25.)
affect the constitution of DHPs. Spruce lignin differs from Zulauf-DHP in a lower content of pinoresinol units and cinnamyl alcohol groups, and in a greater content of P-aryl ether units, a-carbonyl groups, and etherified guaiacyl residues. Nimz and Ltidemann 1311 also investigatedacetylatedlignins and DHPs. Acetylation makes it not only easy to assign signals, but also has the advantage of increasing the solubility of lignin preparations (Fig. 9). Gagnaire and Robert (321 studied a DHP polymer model of lignin that was synthesized by enzymatic dehydrogenation of coniferyl alcohol enriched to 90% in "C on the benzylic position. Gated proton decoupling and selective proton irradiation were used to facilitate assignment of the difficult "C, signals of the DHP. C,, atoms of various structural units, such as vanillin, vanillic acid,coniferylalcohol,cinnamaldehyde. @ - S , p-p, and p-0-4 dilignol units, and the C,, involved in benzyl etherbonds in p-0-4 dilignolstructures, were assigned. Obst and Ralph [33] have tried to determine the relative syringyl/guaiacyl ratios for hardwood lignins, and the following rcsults wereobtained. The syringyUguaiacyl integrated peak area ratio for red oak fiber MWL is I .69, and that for white birch fiber MWL is 2.28. Lapicrer and Monties 1341 estimatedeasily the ratios of syringyl/guaiacylfor hardwood lignins using the signal intensities of C-2 plus C-6 for each from the conventional NMR spectra.
120
Sakakibara and San0 3
19
6
FIGURE 7
33
a
5
24
29
33 34
L 4a
2
FIGURE 8
34
"C NMR spectrum of spruce MWL. (From Ref. 29.)
3 38
2a
22
"C NMR spectrum of birch MWL. (From Ref. 29.)
40
Chemistry of Lignin
121
TABLE 3 "C-Chemical Shifts (6) in ppmfrom TMS and Relative Intensities Spruce MWL (Fig. 7) and Beech MWL (Fig. 9)
of Acetylated
~
Beech, Signal no. 1
2 2a 3 3a 3b
4 4a 5
Spruce, PPm (intensity) 194.9 192.3 179.5 171.4 (159) 170.5 (95) 169.5 (34) 162.1 153.5
6 7 8 10
15 1.4 ( 5 5 )
11
140.8 137.7 (15) 136.7
12 13 14 15 16
17
149.1 148.3 145.4
134.1 (14) 132.4 (26) 129.3 (17)
18 19 20 21 22 23 24 24a 25a 25 26 27 28 29
123.6 (98) 120.7 ( 122) 118.8 (86) 1 16.5 112.9 (133)
30a 30 30b
76.5 75.5 (48) 74.8 (53) 73.3 (25) 72.6 (18) 70.0 (27) 68.3 ( 19) 66.2 (56)
31a 31
32a 32b 32
33a
90.1 88.5 86.3 85.4 83.6 80.7 (60)
PPm (intensity) 195.2 (161) 192.6 178.8 171.7 (161) 171.0 (161) 170.0 162.3 158.7 153.8 (197) 152.0 148.7 144.9 140.4 137.9 136.4 ( 1 9) 136.0 (28) 133.8 (34) 132.6 129.3 123.3 120.5 (31) 118.8 116.5 112.4 (35) 106.9 (45) 105.0 (222) 101.4 88.7 86.7 83. I 81.4 (157)
Assignment a-CO and y-CH0 in cinnamaldehyde a-CHO CO in primary acetoxyl CO in secondary acetoxyl CO in aromatic acetoxyl B(3). C3/5, C(3/5), D M , D(3/5), C,, in cinnamaldehyde A(3), A4, B4 B3 A3 C-4 in B-ring in cyclic p-5 (dehydro diconiferylalcohol acetate) A(4), B( 11, D( 1 ) D4 c 4 , C( 1) D1 BI, Cl A l , C/? in cinnamaldehyde C(4). D(4), C-l in cyclic p-5, C-2/6 in 17hydroxyphenyl ring 4 5 ) . B(5) A6,B6 AS, A(6), B(6) B5 A2, A@) C(2/6), D(2/6) C2/6, D2/6 C,, in cyclic p-S C,, in p-p (pinoresinol acetate)
73.3 (42) 72.6 (48)
C, in GOA (guaiacylglycerol-P-arylether acetate). C,,,,, in a$-diarylether C,, in p- l ( 1,2-disyringylpropane-1 ,3-diol acetate) C,, in GOA C,, in GOA (diasteromer) C, in open p-/?(dibenzyltetrahydrofuran) C, i n p-p
66.0 64.3 ( I 16)
C, in cyclic p-5 and cinnamyl alcohol acetate C, in p-l and a./?-diaryl ether
77.1 (36) 75.5 ( I 19)
55.4
Sakakibara and San0
122
TABLE 3
Continued
~~~~~~~
~~
Signal no. 33 34 35 51.4 35a 36
~
~
~
Spruce, PPm (intensity)
Beech, PPm (intensity)
64.1 (133)
41 .O
6 3 . 3 (197) 5 6 . 4 (255) 55.4 51.3 41.2
20.5 (255)
20.5 (255)
(255)
56.4
40
~
(11)
6
Assignment C, in GOA OCH3 C,, in 0-0 C,in p-1 and p-5 C,, in open p-p CH, in acetoxyl
I
A :R,=H.
0~~
R1 OR
R~=Ac B : R,=H, R H k y l C : Rl=OMc, RFAC D : R I S M C , Rl-
(R = alkyl or Ac) Source:
Ref. 34.
A
A
Ace t y 1a t e d SPRUCE MWL "quant i t a t i v e "
170
150
Acetylated SPRUCE MWL
"routine"
170
150
100
Chemistry of Lignin TABLE 4
123
Formulas forMilledWoodLignins
Wood species
Reference formula Methoxy-free C, formula
Spruce
Beech
111.
ANALYSES OF STRUCTURAL ELEMENTS IN LIGNIN
A.
Formula of Milled Wood Lignin (MWL)
Some representative formulas of milled wood lignins from soft- and hardwoods are shown in Table 4 135-371. These values vary according to the source and nature of the lignin preparations, for instance, wood age, preparation conditions of MWL, carbohydrate contamination, accuracy of determination, and so forth. The differences between species of hardwoods are especially remarkable, arising from the original differences in the nature of the protolignins. In Table 4, the extents of dehydrogenation and additional water per phenylpropane unit without the methoxyl group are shown. The oxygen atoms, excluding the two inherent in the p-hydroxycinnamyl alcohol moieties, are those from water molecules added to the quinonemethide and are shown in parentheses.
B.
End Groups with Unlinked Side Chains
As the lignin macromolecule is thought to be formed by the dehydrogenation of cinnamyl alcohols (1-2), it is probable that unsaturatedsidechains(-CH=CH-CH20H) are retained asendgroups. It is wellknown that Freudenberget al. [36] obtainedmany dilignols and trilignols with cinnamyl alcohol side chains(-CH=CH-CH,OH) and two dilignols with cinnamaldehyde side chains (-CH=CH-CHO) in the enzymatic dehydrogenationproductsfrom coniferyl alcohol (L). Similar lignols withthese side chains were also isolated by the mild hydrolysis of protolignins [38,39]. Treatment with phloroglucinol-HC1, known as the Wiesner reaction, is a typical color reaction of lignin, forming a violet cationic chromophore (Fig. 10). The reaction mechanism involving the coniferyl
OR (6) R= H or alkyl
(z,
FIGURE 10 Colorreaction of coniferyl alcohol groups.
I
124 San0
and
Sakakibara
aldehyde function was elucidated by Adler et al. [40]. From this color reaction, Adler et al. [42] estimated coniferyl aldehyde groups to be 2-2.5% in spruce lignin and 3-4% in BL of western hemlock. Later, however, the A&,, method indicated that 3-4% [42] and 3% [45] cinnamyl alcohol groups are present in spruce MWL. The existence of a small amount of coniferyl alcohol groups i n the lignin molecules was demonstrated with a color reaction exploited by Lindgren and Mikawa [44]. Coniferyl alcohol (1)and its 4-0-methyl ethers (8) react nitrosodimethylnitrile after tosylation, giving the p-dimethylaminoanilide of styrylglyoxalnitrile (y), which isredin color (maximum 475 nm), via intermediate (Fig. 11). Coniferyl alcohol groups in spruce lignin were estimated to have the same content as cinnanlyaldehyde moieties (2%) by this color reaction. The presence of cinnamic acid-type side chains in wood lignins is negligible, even to a lesser extent than in glass lignins [45,46]. Glycerolsidechains in lignin molecules are still beingdebated,buttwo p-0-4 dilignols with glycerol side chainswere isolated by hydrolysis with dioxaneandwater [47,48], extraction with water [49], and also by treatment with metallic sodium in liquid ammonia [50].A model experimentsubstantiated the fact that the glycerol side chain could not beformedfroma p-0-4 structure by hydrolysisunder neutral or acidic conditions [51]. Higuchi et al. [52] detected small amounts (0.03-0.6%) of three arylglycerols in the enzymatic dehydrogenation mixture of p-hydroxycinnamyl alcohols. This finding supports the contention that glycerol side chains can exist in the native lignin macromolecules, but the presence in lignins is rather insignificant because of formation of only small of formaldehyde by periodate oxidation 153,541. Dilignolsbearingo-propanolsidechains (-CH,-CH,CH,OH) havebeen isolated from the dioxane-water hydrolysate of protolignin [55]. The aglycones of glycosides (11)and (g) that were isolated as extractives from scotch pine (Pinus .syhwrris) were optically active [56]. On the other hand, the hydrolysis product is not optically active, suggesting that it may originate from lignin. The NMR spectra of MWLs show unknown proton signals in the higher-field region (6 0.38-1.58), and Ludwiget al. [IS] estimated the content of correspondingproton content to be 0.2-O.4/C,C3. The protons in this range may correspond to those of y-methyl and methylene. Compound (11) may represent one of these side chains. Presumably, some disproportionation may occur, or a reducing mechanism similar to that in the case of wood extractives may be operative during biogenesis.
(m)
(m)
HC
l
-0 I
HC
R7 O
O M e
R3
Cu1,
R,=H. R:=H
,Rs=OMe
Chemistry of Lignin
bo"
125
FH20H
OMe OMe
r I
OMe
aniline
OMe
OMe
0
Ce,pAmethylanin&lidc
of
styrylglyoxylnimlc ,red (mm.4751x11)
FIGURE 11
Color reaction of coniferyl alcohol groups.
known. Adler and Marton [59] determined carbonyl groups spectrophotometrically through the reduction of various aldehydes and ketones in guaiacylpropane structures with sodium borohydride in alkaline solution. The Acr changes in the adsorption spectra were treated by means of borohydride reduction curves, where the carbonyl compounds are reduced to the corresponding alcohols with different rates. Then, the A&,. curves of methylated and unmethylated spruce MWLs were qualitatively and quantitatively analyzed by Comparison with the A&, curves of modelcompounds. The results allowed the values for various carbonyl contents per OCH, in MWL to be estimated as shown in Fig. 12. In addition to these carbonyl groups (in total, 0.09-0.1 I/OCH,), unconjugated carbonyls may exist by as much as the same amount. The types of the unconjugated carbonyl groups in the lignin molecule have not been elucidated completely as yet, but some of this is due to glyceraldehyde-P-aryl ether substructure which the side chains have been eliminated. Examples of and As,, curves are shown in Figs. 13 and14.
D. Phenolic and Aliphatic Hydroxyl Groups The free phenolic groups have been quantitatively determined by various methods, such as the A&, method of Aulin-Erdtman as described in the section on UV spectra, conductometric or potentiometric titration in aqueous [60,61] or nonaqueous [62,63] solutions, reaction with dinitrofluorobenzene [64], reaction with sodium periodate [65], methylation with diazomethane [66], NMR spectra [18,19,27], etc. Adler and Hernestam [65] treated guaiacyl model compounds (Q) with sodium periodate, giving the corresponding o-quinones (@), which were determined quantitatively
C.!'& OMe
OH
OMe
/o
' OMe
OH
I
n
m
4.01/0CH3
0.0310CH3
O.OI/OCH,
FIGURE 12 Various carbonylgroupsin
&
' OMe
carbonyl
/o N 0.05-O.WOCH3
V 0.09-0.11/OCH3
lignin. (From Ref. 59.)
unconjugated
126
Sakakibara and San0
& x10 - 3
NaBH4 NaOH
0.01N
0 (b)
I
250
I
300
350 my
FIGURE 13 (a) Absorption curve of a-guaiacoxy-p-oxy-propioveratroneand the reduced one with NaBH,: (bj AF, curve.
by spectrophotometry (Fig. IS). From these results, it was estimated that 30% of all guaiacy1 units have freephenolichydroxyls.Thestructural units with afree phenolic group react with I-nitrosonaphthol to give compounds with a maximum absorption at SOS nm. Okay [67] has determined free phenolic hydroxyl groups in lignins by the application of this reaction. However, the values obtained by these methods do n o t always agree with each other, because they are not equally effective with all types of phenolic hydroxyls. For instancc, the AE, method cannot be used for determining hindered phenolic hydroxyls. It has been claimed that the potentiometric titration with sodium colamine in ethylenediamine could be used todetermine all freephenolicgroups (621. but i n fact, the values obtained are somewhat larger (0.33-0.34/OCH, in spruce MWL) than they should be because of the cleavage of benzyl aryl ethers. Furthermore, the oxidation with periodate
127
Chemistry of Lignin
I
4,O
UV absorption (neutral)
log E.
3.0
2.0
1 .o
250
300
350
1,m p
400
FIGURE 14 UV absorption in neutral solution and ionization A&-curves: a, a ' , untreated MWL; b, b', hydrogenated MWL; c, c', NaBH,-reduced and subsequently hydrogenated MWL.
[65] is applicable only to guaiacyl lignins (0.30/OCH3 in spruce MWL). The 'H NMR approach is simple and can be used to determine the protons of phenolic acetoxyl groups in acetylated lignins, but the accuracy is not satisfactory (0.27/OCH3 [ 191 and 0.29/OCH3 [ 181 in spruce MWL). Furthermore, Li and Lundquist [27] estimated by the NMR spectrometry of lignins at 400 and 500 MHz using DMSO-d, that phenolic groups in spruce MWL are 0.24/Cy, of which about 20% originate from phenolic groups in biphenyl and diary1 ether substructures, and those in birch MWL are 0. I WCy, in which the proportion in guaiacyl and syringyl units is 3:2. Robert and Brunow [68] have estimated the phenolic hydroxyl groups in MWL by "C NMR. Chang et al. [69] have determined the phenolic hydroxyls in cellulolytic enzyme lignins fromsweetgumandspruceandobtainedsomewhatlowervaluesthanthose in
.Q OH u1)
-Q N~OJ
OMe
+
CH30H
0
0 W
FIGURE 15 Oxidation of guaiacyl nucleus with sodium periodate.
nces
e
Sakakibara and San0
128
TABLE 5 Phenolic Hydroxyl Groups of Spruce MWLs Method Phenol-OH/OCH,
0.29, 0.27 0.27, 0.24 0.20 0.30 0.33-0.34 0.33 0.15-0.20
'H NMR NMR 'H "C NMR Periodate Titration Aminolysis
t18, 191
W , 271 L681 ~651
[621 [701
"Cellulolytic enzyme lignin
correspondingMWLs, 0.09-O.13/C,C3 for sweetgumand 0.15-O.20/C6C, for spruce. MAnsson1701 has developed a new method for the determination of phenolic hydroxyls in lignins by acetylation and subsequent selective aminolysis with pyrrolidine. The phenolic hydroxylgroupcontentsobtained so f a r are summarized in Table 5. Robertand Brunow 1681 also estimated the different types of hydroxyl groups in lignin preparations usinga "C NMR pulse sequence that involves gated proton decoupling. The carboxyl carbons in acetylated samples give signals that allow three different types of hydroxyl groups to be distinguished. The results obtained are shown in Table 6. Recently, the evaluation of 'H-, '.'C-, "P-NMR [71], FTIR (721, and wet chemical methods has been made to determine the contents of total hydroxyl, phenolic, and aliphatic hydroxyl groups in lignins [73], reporting that FTIR or 'H-NMR spectroscopy is recommended for routine determination of phenolic OH/aliphatic OH ratios, and that "P-NMR affords the determination of the stereochemical configuration of p-0-4 linkages and the phenolic OH contents due to G and S units.
E. Condensed Units Potassium nitrosodisulphonate, known as Fremy's salt, oxidizes p-substituted phenols to o-quinones. For example, 4-propylguaiacol is oxidized to methoxy-5-propyl-o-quinone (16) (Fig. 16) 1741. The guaiacyl units (B) possessing an unsubstituted 5-position are called "uncondensed," and the units that carry C-C or ether bonds at this position are called "condensed." Adler and Lundquist applied this oxidation to estimate uncondensed units in lignin. The o-quinone (16)formed can be quantitatively determined by means of spectrophotometry. Hereby, it was found that 0.15-0.1 8 units per methoxyl in MWL were uncondensed phenolic units, corresponding to 50-60% of the 0.30 phenolic
(e)
TABLE 6 Numbers of Hydroxyl Groups per OCH, Calculated from the Intensities of Acetyl Signals in Acetylated Samples and Those Obtained by Acetylation and Aminolysis OH Sample DHP Spruce MWL Suruce MWL
OH
Total Phenolic Secondary Primary OH OH
1.32 0.78 l .34 1.26
0.350.73
0.16 0.3 1
0.20 0.33
1681 1681 1701
129
Chemistry of Lignin
c-c-c
c-c-c OMe
OH
0
ui,
0
FIGURE 16 Determination of condensed units by oxidation of guaiacyl nucleus with Fremy’s Salt.
units present; i.e., 0.12-0.15 per methoxyl were presumed to be condensed units from the difference, corresponding to 40-50%. However, as the oxidation with Fremy’s salt can onlybeapplied to the units witha free phenolichydroxyl, no information is obtained about etherified units. By means of ‘H NMR spectroscopy, about 45-50% condensed units [18,21] and less amounts of them (35% and 30% for spruce and birch MWLs) [22] have been estimated. The latter were calculated by combination of the amounts of OCH, determined by the bromine method and of aromatic protons by ‘H NMR of hydrogenated MWLs using p-nitrobenzaldehyde as an internal standard.
F. p-5 LinkedUnits P-5 linkage units are represented by the phenylcoumaran structure (B).Dehydrodiconiferyl alcohol was isolated by the 0.5% HCl-methanol treatment of spruce wood by Freudenberg et al. [75], and phenylcoumaran lignols were isolated through dioxane-water hydrolysis [76,135]. Adler et al. [77] found that dihydrodehydrodiconiferyl alcohol (g) and its phenyl methyl ether are converted to the corresponding phenylcoumarone (B)in 90% yield after 20 h of heating in 0.2 M HCI (Fig. 17). The phenylcoumarone with its stilbenoid conjugationshowsastrongabsorption at 310 nm,and the phenoliccompoundgivesa Asi maximum at 338 nm. This conversion provides characteristic difference curves. Quantitative evaluation of the spectra indicated that the spruce MWL contained 0.1 1 dimeric structures per methoxyl that can be converted into phenylcoumarone moieties on acidolysis. When the MWL was methylated with diazomethane, the number of phenylcoumarone moieties formed on acidolysis was about 0.08. This means that the MWL contains about 0.03 P-5-condensedbut not ring-closeddimeric units (E), which,however,are converted into phenylcoumarone moieties closure on acidolysis. Therefore, the number of phenylcoumaran moieties (18) in the MWL is calculated to be 0.08 per methoxyl.
(B)
G.
Benzyl Alcohols and Benzyl Ethers
Benzyl alcohols and benzyl ethers are two of the most important functional groups in the lignin molecule for various reactions involving pulping. The determination of these groups is therefore especially significant. Various benzyl alcohols, dilignols, and tri- and tetralignols have been isolated by mild hydrolysis and hydrogenolysis, as will be described later (see Section W). However, noncyclic benzyl ethers are very difficult to isolate from the degradation products of lignin because of the labile nature of these ether linkages. Adler and Gierer C781 treated lignin with methanolic hydrochloric acid and concluded that the total amount of benzyl alcohol and noncyclic benzyl ether was about 0.43/OCH3 in spruce MWL, becausecyclicbenzylethers are not methylated.Benzylalcohol units withfree
130
Sakakibara and Sano CH2CH2CH20H
‘acidolysif
OMe
*
(O.2N Ha in dioxanc-
H20.2Oh.rdlux)
8-
OMe I
c-
0
OMe
OMe OH
OH 0
uz)
c-c-c
c-c-c
OMe
I
$L0
CHOR
OH
OMe OH
@OM. OH
FIGURE 17 Determination of p-5 linkedunitsby
acidolysis.
phenolic hydroxyls ( 2 0 ) have been determined with the quinone monochloroimide (2) color reaction by Gierer [79,80] (Fig. 18). Adler et al. [81,82] found that p-alkoxybenzyl alcohol (3) is oxidized to the corresponding aryl ketone ( 2 5 ) withdichlorodicyan-pquinone (2), which is reduced to (Fig. 19).The a-ketone (g) formed was determined spectrophotometrically, and a value of 0.16/OCH3 was obtained. Thus, p-hydroxybenzyl alcohol units constitute 0.05/OCH3, esterified benzyl alcohol 0.10/OCH3, and benzyl ether (except cyclic ether) 0.06/OCH3. Higuchi et al. [83] estimated a-aryl ethers to be 0.070.09/C,C3 from the results of the acidolysis of MWLs of bamboo, beech, and Thuja stundishii. Freudenberg et al. [84] estimated these groups by cleaving the benzyl ethers with
(B)
OMe OH
OMe
0
quimemonochlorimidc
indophenol
A mal. 6x)nm
FIGURE 18 Reaction of quinonemonochlorimide
(U)with p-hydroxybenzyl
alcohol groups (g).
z
131
Chemistry of Lignin R
NC
OMe
0
OMe
OH
OMe
W
0
Cl
OMe (21)
dichlomdicyan-pquinonc
FIGURE 19 Reaction of dichlorodicyan-p-quinone (g) with p-alkoxybenzyl alcohol groups (g).
sodium colamine in ethylene diamine solution. Besides this reaction, cleavage with methanolic hydrochloric acid after methylation and sulfonation were also applied [85].From the results, it was estimated that p-hydroxybenzyl aryl ethers amounted to about 0.041 OCH, and p-alkoxybenzylaryl ethers 0.06-0.09/OCH3. These results are summarized in Table 7. The benzyl alcohol units have also been determined semiquantitatively from NMR spectra as 0.33/OCH, [ 181, 0.32 [19], 0.31 [68], or 0.29 [22] in spruce MWL and 0.45 [22] in birch MWL. Gagnaire and Robert [32] have estimated the benzyl alcohol content to be 0.31/OCH3 from the "C NMR of DHP.
H. p-0-4 LinkedUnits Arylglycerol-p-aryl ether units (g) and (g) belong to the most important substructures in lignin molecules. It is well known that Hibbert's ketones are formed from these linkages in lignin during alcoholysis (Fig. 20). Adler et al. [86] found that acidolysis liberated about 0.3 phenolicOWOCH, in MWL andreportedasimilarnumberofterminalC-methyl groups characteristic of the side chains of Hibbert's ketones (31-34). The results indicated that p-0-4 units (2-2) may be 25-30% of all phenylpropanes. From 'H NMR spectra, Lundquist estimated later that 40-50% of birch lignin units [24] and 30-50% of spruce lignin units [25] are attached to an adjacent unit by a p-0-4 linkage. Miksche et al. have studied the oxidation products of lignins and have estimated the content of p-0-4 units in birchandspruceMWLstobe0.62 [87] and 0.49-O.51/C,C3 [88], respectively, by multistage oxidations.
TABLE 7 BenzylAlcoholandBenzylEtherContents Spruce Lignin
in
Hydroxyl ~~
p-Hydroxybenzyl alcohol p-Alkoxybenzyl alcohol p-Hydroxybenzyl ether ether p-Alkoxybenzyl
0.06
U311
0.05
V91
0.10 0.02 0.04
L811 l811 1841
0.06 0.06-0.09
P11 [g41
132 Sano
and
Sakakibara
cH20pb I
CH2OI I ?leo
I
H?--0
HC HC2 0-p oO
HC-0-C
HC-OH
I
b
C
-
O
b
II
CH
OMe
OMe OH
0
0
0
H,Oo
OMe
'
OH
0 0.30/C&
OH
Formation of Hibbert's ketones by acidolysis of p-0-4 units.
FIGURE 20
1.
p-l LinkedUnits
Nimz [S91 first isolated diarylpropanediols (g) from the degradation products of spruce and beech protolignins by mild hydrolysis. The mechanism of formation of the p-1 linked units (g) has been proposed by Lundquist and Miksche [90] as shown in Fig. 2 1. Phenoxy radicals (2)and maycoupletogive the cyclohexadienone (E),which maybe cleaved, giving the p- 1 linked compound (B) and glyceraldehyde-2-aryl ether (S). Lundquist and Miksche estimated the content of this aldehyde (0.3%) from the yield of methylglyoxal during acidolysis of lignin.
(x)
F
d
O
H
8,.""'
R1
J.
BiphenylStructures
Aulin-Erdtman [91] found that the mostobvious effect ofincreasing the pH of lignin solutions was a higherabsorption in the UV spectrumabove 300 nm.Thisabsorption band is characteristic of biphenyl structures. The number of hydroxy-biphenyl units in
133
Chemistry of Lignin CH2OH I
H?-OAr
HC-OAr
*
I
0CHOH
$
-
~ H O HOMe %,H'
I
I
H?
HrH
CH20H
CH20H
OMe +
-
I
CH
OMe
Q 0O M e
0
0
up,
H20
Hys;H
KMe I
+
OH ue,
FIGURE 21
CH0 I
HC-OAr I
CH20H
0
Formation mechanism of diarylpropanol on biosynthesis of lignin. (From Ref. 90.)
black spruce BL was estimated using a twice-reduced difference curve at 325-340 nm. The results obtainedindicated that there are 0.05/OCH3 biphenyl units in BL. Pew [7] estimated a still higher value, 0.25/C6C,, for spruce MWL. Miksche et al. estimated values of 0.045 for birch lignin [87] and 0.095-0.11/C,C3 for spruce lignin [88] from oxidation product yields. Nimz [38] estimated 0.O23/C,C3 for beech lignin. Between these estimated values there are considerable differences. From the permanganate oxidation products [92], in additionto the mainbiphenyl unit, 5-5 5-6 (g), 5-1 (Q), and 6-6 (g) type biphenyl units are presumed to be present, but have not been isolated from the products of hydrogenolysis and hydrolysis, indicating that they may give rise to minor products.
(e),
COOH
Me0
OMe
OMe OMe
K. 4-0-5 Linked Units Freudenberg and Chen [92,93] first isolated 4-0-5 (E,%) and 1-0-4 (g,%) type diphenyl ether compounds by permanganate oxidation, and then Larsson and Miksche [94] isolated two 4-0-5 type oxidation products (S,@) Nimz et al. [95] isolated a guaiacyl-syringyl dilignol with a 4-0-5 linkage (168) by treating beech lignin with thioacetic acid, followed by reduction with Raney nickel. Yasuda et al. [96] isolated a guaiacyl dilignol with a 4-
and
134
Sakakibara
San0
(m)
0-5 linkage from the hydrogenolysis products of larch compression wood lignin. Miksche et al. estimated the frequency of 4-0-5 linked units from the yield of permanganate oxidation products to be 0.035-0.04 for spruce lignin [88] and 0.065/C6C3for birch lignin [87]. On the other hand, Nimz et al. [95] reported 0.O15/C,C3 for beech lignin.
L.
p-p LinkedUnits
p-p type structures are involved in lignans represented by pinoresinol (44) and syringaresinol Of unitslinked in this way, (@ wasfound to be formed by enzymatic dehydrogenation of coniferyl alcohol (L) [97]. However, with the exception of the finding that pinoresinol is detected in the products formed by room-temperature methanolysis from spruce protolignin [75], isolation of that compound from lignin degradation products has failed. Syringaresinol,on the otherhand,was isolated from the productsof the mild hydrolysis of beech wood by Nimz [98]. Omori et al. [99] also isolated syringaresinol and episyringaresinol from Fraxinus mandshurica by hydrolysis with dioxane and water. Further, a dioxa-bicyclo-octane composed of guaiacyl and syringyl units (S) [48], dimethoxylariciresinal [ 1001, and a trilignol involving the syringaresinol moiety [99] were isolated, as will be described later. Nimz [95] also isolated compounds with the isolariciresinol ring andwith the tetrahydrofuran ring substituted byguaiacyland syringyl units In general, p-p linked units are involved much more in hardwood lignin than softwood lignin. Lundquist [25] estimated a low content for pinoresinol units (0.02-0.03/OCH3) in spruce MWL from its 'H NMR spectrum. Miksche et al. also estimated 0.03-0.05/C,C3 p-@units for birch lignin [87] and 0.O2/C,C3 forspruce lignin [88].OgiyamaandKondo [ 1011 estimated the content of pinoresinol structures as 0.05-0.10/OCH3 for softwood lignin from the yield of the di-y-lactone formed by nitric acid oxidation.
(e).
(m).
R2
HO$..(
OMe
H0
M. p-6 and p-2 Linked Units p-6 and p-2 linked units are presumed to exist in the lignin molecule, as metahemipinic (p) and hemipinic ( 7 8 ) acids were detected in the products of permanganate oxidation [92]. This substructure was first isolated as a dimeric phenylpropane from the hydrogenolysisproducts of spruce lignin bySudo et al. [102].Yasudaet al. [l031 isolated p-6 linkedphenylisochroman (E) from larch lignin by hydrogenolysis. These p-6 linked units may energetically form more easily an a - 0 - y linked phenylisochroman ring than an open structure, but it is not clear whether the p-6 linked units should always exist as a closed ring or not. Miksche et al. estimated the content of p-2 and p-6 linked units to be 0.015-0.025/C6C3 for birch lignin [87]and0.025-0.03/C6C3forspruce lignin 1881, respectively.
135
Chemistry of Lignin
N. Other Linkage Units Freudenberg et al. [93] isolated anaromaticacidinvolvinga 1-0-4 linkagefrom the permanganate oxidation products of lignin, suggesting the existence of 1-0-4 linked lignols (E,%), but such a compound has not been isolated as a phenyl-propanoid as yet. Nimz [95] isolated cyclolignan-bearing p-p and a-6 linkages from beech lignin by thioacetic acid degradation. This structure was postulated by Freudenberg [92] as a precursor of the benzene polycarboxylic acid that was found among the permanganate oxidation products.Nimzalso isolated a-p typecompounds (E) andtetrahydrofurandilignols involving 'y-0-7and p-p linkages Pew et al. [7] have suggested that the diphenyl ether 1-0-4 linkage is formed by side-chain displacement after radical coupling at C, and C,, leading, for example, to an intermediate ( S )in the formation of dioxepin (*), as shown in Fig. 22.
(x)
(m).
W.
DEGRADATION
A.
Oxidation
1. Alkaline Nitrobenzene
Freudenberg [l041 was the first to report that lignin provides a high yield of vanillin (E) by the alkalinenitrobenzeneoxidation. The yield of 20-28% fromspruce lignin proved the aromatic nature of lignin. Later, Leopold [ 1051 studied these oxidation products from spruce wood in detail, also deducing the presence of p-hydroxyphenyl units in softwood lignin (Table 8). Leopold [ 1061 and Pew [ 1071 demonstrated that the side-chain structure has considerable effect on the yields of oxidationproductsfrommodelcompounds. Units having side chains substituted with a hydroxyl at the a-position and vinyltype guaiacyl units give high yields of vanillin, and those with a-carbonyl groups increase the yield of vanillic acid (S). Units bearing alkyl substituents atthe 0-position to phenolic hydroxyl exhibit the highest resistance to oxidation. Substituents at the a-carbon of the side chains and cyclic ether structures such as pinoresinol are also difficult to oxidize. The products obtained by alkaline nitrobenzene oxidation are summarized in Fig. 23. Brink et al. [108,109] investigated the oxidation products (methylated) of white firin detail and reported various compounds besides the products.
(E)
MeO Me0 OH
OH
MeO
OMe OH
OH
m FIGURE 22
W
A mechanism of formation for diphenyl ethers. (From Ref.
0 dioxepin
7.)
OH
136
Sakakibara andSano
TABLE 8 NitrobenzeneOxidationProducts from Spruce Wood Compound
Yield (%)
Vanillin ( 5 4 ) p-Hydroxybenzaldehyde Syringaldehyde ( g ) Dehydrodivanillin ( g ) Vanillic acid (g) acid Syringic 5-Formylvanillic acid (63) 5-Carboxbvanillin (9) Dehydrodivanillic acid Acetoguaiacone (g)
(S)
(a)
(E)
27.5 0.25 0.06 0.80 4.8 0.02 0.1 1.2 0.03 0.05
Source: Ref. 105.
PermanganateOxidation Freudenderg et al. [92,93] heated spruce lignin or spruce wood with 70% aqueous potassium hydroxide in order to bring about hydrolytic cleavage of ether linkages and subsequently protected the phenolic groups liberated by methylation. Permanganate oxidation of the methylated products at pH 6-7 gave veratric acid ( 7 4 ) in a yield of about 8% of the lignin and minor amounts of isohemipinic and dehydrodiveratric acids (g,%). Furthermore, they isolated and identified 19 methoxy-substitutedbenzenecarboxylic acids.
2.
CH0
COOH
R1
R2
F2
71
M
e
O
m
O
M
OH Rl=H, R2=OMe (U) R,=RZ=OMe (12, Rl=Rz=H
0 Rl=CHO R2=OMe 0 R]=COOH, R2=OMe W Rl=CHzOH. RZ=OMe I
R l
OH R=H (hl) R=CHzOH
161)R=COCH3
c66)R=CHzCH2CH20H (42) R=CH2COCH3
FIGURE 23 Alkaline nitrobenzene oxidation products of lignin.
e
Chemistry of Lignin
137
Miksche and co-workers [ 1 10,ll l] found that considerably higher yields of the aromatic carboxylic acids were obtained if the oxidation was carried out by a mixture of sodium periodate and permanganate in aqueous t-butanol with sodium hydroxide at 82°C. Since the product mixture contained appreciable amounts of phenylglyoxylic acids, however, the latter acids were degraded to the corresponding benzoic acids in a secondary oxidation step, consisting of brief treatment with alkaline hydrogen peroxide. The latter method gave well-reproducible results as shown in Table 9. If wood or isolated lignin were methylated and oxidized, the resulting aromatic acids reflected the units in lignin which carried a free phenolic hydroxyl group. Preheating with alkali convertednonphenolic units intophenolic. This is, andfrom the increase in the yields of aromatic acids, therefore, the proportion of etherified units could be estimated [94]. Alkaline cleavage of the ether linkages was performed under conditions for kraft cooking or oxidation with alkaline cupric oxide. The mixture of benzoic acids was finally methylated, and the resulting mixture of methyl esters was assigned by gas chromatography and a combination of gas chromatography and mass spectrometry for quantitative estimation and structural identification, respectively. Table 9 shows the yields of the major acids obtained on degradation of a methylated spruce MWL and of the same lignin which had been subjected to ether cleavage prior to methylation [ 1 1 l]. The results obtained with methylated kraft lignin prepared from spruce wood meal is also included in Table 9, indicating the good reproducibility of the method, and spruce MWL is structurally very similar to the lignin in the wood. Also, pretreatment with NaOH/CuO gave considerably higher yields of most of the aromatic acids than pretreatment under kraft cooking conditions. A total of 40 aromatic acids has been identified in the reaction mixture obtained on oxidation of methylatedspruceMWLwhich had notbeensubjected to ether cleavage [ 112,1131. From spruce lignin, hemipinic acid biphenyls (4J-g,@-@), diphenyl ethers (87-90), andbenzenepolycarboxylic acids weredetectedbesides veratric isohemipinic (E), and metahemipinic acids as summarized in Fig. 24. More abundant aromatic acids were obtained from softwoods were (T),(g),and (@-g), and
(z), (z), (z,2),
TABLE 9 Yields of Methyl Esters (in mg/100 mg of lignin) Obtained by Oxidation of Methylated Spruce Lignin
MWL methylated
2.0
0.75 0.70.25
11.2
1.1
I S5
MWL treated with 2 M NaOH/CuO and methylated
29.8
5
0.7
1.1
2.1
5.0
MWL treated with kraft cooking conditions and methylated
21.4
0.5
21.3
0.5
3.6
I .75
Kraft lignin from wood meal methylated
Source:
0.45 Ref. 167.
0.6
5.93.4
I .65
6.0
(B),
138
Sakakibara and San0
RH
RQ C O O H
OMe R2
R1
COOH
OMe
(HL) R=H
0 R=OMe 0 R=COOH
COOH
COOH
I
Me0
Me0 R=H @&)R=OMe
OMe
Q
OMe
R
OMe
OMe
COOH OMe
@ Rl=Rz=H &l (81) RI-+Me ,Rz=H (86) RI=RflMe
OMe (8e) R=H
@Q) R=OMe
Me0 OMe
ceu
COOH
COOHA I
Me0 V
O
koM ‘’ ’ COOH
I
OMe M
eMe0
COOH COOH
Me0
OMe
/
OMe
OMe
OMe
0
OMe
W
OMe
W COOH
COOH COOH Me0 Me0 OMe
0 0
FIGURE 24
OMe OMe
0
OMe
Permanganate oxidation products of lignin.
(z,z),
those from hardwoods were (E),(Q), and (86-83). Other aromatic acids appear in small amounts (around 0.1 % of the lignin) or in traces (>O. 1%). The diaryl ether (g) and the biphenyl acids ( g )being , monocarboxylic acids, originated from substructures from which one of the side chains has been detached. The tricarboxylic acid (3) is one of the examples indicating a mixed radical coupling (coniferyl and p-coumaryl alcohols) and, analogously, the diaryl ether ( g ) is derived from a substructure formed from a sinapyl and a coniferylradical. The trimethoxylated ring in the trace constitutents were remarkable.
Chemistry of Lignin
139
The methoxyhydroquinone ring in these acids may be have been formed by reduction of a methoxy-p-quinone moiety which seems to be the hydrolysis product of a 2,4-cyclohexadienone diary1 ketal structure such as (3) being formed by dehydrogenative coupling [ 1131. It points to the presence in lignin of a methoxyhydroquinone.
B.
Hydrogenolysis
Previously, the hydrogenolysis of lignin wasstudiedtoproducechemicalsandalsoto obtain structural information. Recently, protolignins have been subjected again to catalytic
YHOH YHOH
R R=OMe R=H
OH Cez, R I = R 2 = b = H or OH R3=H or OMe
OH
0
Me0Q O M e OH
OH
CH2 CH20H
OMe MeO’
0
OMe (ep) R=H or OMe OCH2CH2OH
MeOQ
0
O M e OH
umz, CH2R
YH2OH
I
y
HC-
2
H&”O“CH I
MeO OH OH
OMe OMe
cuL1)R=H or OH
OMe
OH UM) R=H
or OH
OMe
MeO
OH
W
FIGURE 25 Products obtained by mild catalytic hydrogenolysis of protolignins with copper chromium oxide at about 240°C.
140 San0
and
Sakakibara
Me0 OH OH
R3
uQ6)R,=R2=H or OH R3=H or OMe
OMe
Q O M e OH
R=H or CHIOH
oc'o"-
y
m6
HOH27
2
7H2
H?-
CH2
OMe OH
OH
Me0
OC'O,
?H2
H?-
YH
CH2 /
OMe
/
OMe
OH
uu OH
FIGURE 25
W
Continued
hydrogenolysis under conditions at about 240°C with copper chromium oxide, leading to the isolation of various dimeric and trimeric compounds (94-111) besides a substantial amount of monomers [102,103,114-117,1211. The lignols isolated are summarized in Fig. 25. Hydrogenolysis cleaves most of aryl-alkyl ethers, but a few of these linkages remain intact as seen in compounds (95 - R, = OH, 96). Compound (96) - has an a-hydroxyl that
HC-0
141
Chemistry of Lignin R
I CH II CH
CH20H I
l CHOH
HOH27 Q O M e HOH2C HC-0 I CHOH
I
R
$$,
I
HC-
0
OMe
OH R=H or OMe
OH
0 Rl=CHCHCHzOH Rz=H
G OH O M e
R$
OMe
u1z) R,=CHCHCHO
R2=OMe
0 R,=CHzCH?CHzOH Rz=OMe
FIGURE 26
Products obtained by mild hydrolysis of protolignins with aqueous dioxane at 180°C.
142 San0
and
Sakakibara
(m)
(m)
has quite exceptionally remained unaffected. Compounds [ 102,1141 and [ 1031 should give metahemipinic acid (2) by permanganate oxidation of methylated lignins. Compound was isolated from the lignin of larch compression wood, but its occurrence in normalwood lignin isalsoprobable. Itcanbeconsidered that compounds (101,102) could be derived by reductive cleavage from pinoresinol and (E), respectively. However, a model experiment indicated that the alkyl-alkyl ether of the tetrahydrofuran ring is very stable toward hydrogenolysis, and the starting material (g) was almost completely recovered [ 1151. This fact suggests that compounds (E) may not be derived from compound after all, and these linkagepatterns may exist independently in lignin molecules. Compound (g) was isolated from the hydrogenolysis products of hardwood protolignin [ l 161, indicating that the alkyl-alkyl ether is fairly stable against the reductive cleavage. Compound (96)contains a 7-0-4 linkage [ 1171 so far not known. It is, however, very probable that a p-0-4 linkage can be enzymatically rearranged to a y0 - 4 linkage. The existence of 7-0-4 linked units waspostulatedatan early stage by Freudenbeng [ 1191 in 1933 without experimental support, but later he abandoned the idea. Subsequently, in 1960, Brauns et al. [l201 proposed the same substructure. However, this linkage pattern may be a minor one in the lignin macromolecule. Compound (F), which was isolated from hardwood protolignin [ 1211, has a heterocyclein the molecule involving a 4,5-dihydroxy-3-methoxyphenylmoiety. Compounds ( I 10,111) are trilignols with a y-lactone. They have no optical activity. The IR spectra of MWLs show a small shoulder at 1760 cm”, indicating the existence of y-lactones. The facts indicate that p-hydroxy cinnamic acids are also involved in the radical coupling scheme after enzymatic dehydrogenation. Nimz [95] cleaved protolignin from beech wood with thioacetic acid using boron trifluoride as a catalyst followed by reductionwithRaney nickel toproducemanydimericcompounds.Theproductswere somewhat different from those formed by hydrogenolysis.
(m)
(e)
(e)
C.
MildHydrolysis
1. Hydrolysis withWater
Nimz [125-1291 percolated extractive-free wood powder with water at 100°C for several weeks (“mild hydrolysis”), showing that beech wood loses about 40% of lignin, while only 20% of lignin in spruce wood goes into solution. From hydrolysis products of spruce were isolated eight dilignols, two diastereoisomeric trilignols, and one tetralignol: guaiacylglycerol-p-coniferyl ether [ 1261, a trilignol involving p-0-4 and p-1 linkages (123)[127], a tetralignol involving one 6-1 and two p-0-4 linkages (125)[ 1271, guaiacylglycerol-p-guaiacylglycerol ether [ 1261, and guaiacylglycerol-p-coniferylaldehyde (M)[ 1281, and from beech were isolated syringaresinol (g) [98] and three diarylpropanediols (115)[89,123].
(e) (e)
2. Hydrolysis with Dioxane and Water Sakakibara et al. [ 130-1391 found that 40-60% of lignin can be dissolved by treating wood powder with a dioxane and water (1: 1) mixture at 180°C. The many degradation products are almost the same as those obtained by Nimz (Fig. 26). Arylglycerol-p-aryl ether (114) [48], three diarylpropanediols [ 133,134,551,thephenylcoumarans (1 17,122) [76] and [ S ] , syringaresinol(45) [99], adilignol with an a-carbonyl group (g) [loo], the trilignols (122)[135], (123)[133], (124)[100,136], and the C6-C3-C3 lactone (Fig. 27) [ 1371 were isolated and identified, besides considerable amounts
(m)
(m)
(x)
143
Chemistry of Lignin
OH OH
M e o ~ o M e
+
H2?/"CH MeoQoMeI
Me0QOMe OH
OH
0
OH OH M e O A O M e
M e o ~ o M e
CH20H I
'CH
H2qA0"CH II
I
(b) R
6 0
HC$/C" I
CH20H
HCI
I
CH I
CH l
Me0
OMe+ Me0
OMe
OMe
0
OMe
0
/
0
J +H20 OMe H o H q G O H HOHC I
R Q OH O M
OMe e
R=H or OMe FIGURE 27
Proposedformation
(g). (From Ref.
+
Meo6
H2?C ,"H
I
HC-
CH
I
I
O+C-~-CH2 UZL)
mechanism of compound for biogenesis of substructure unit
137.)
of monolignols. A compound (M)with an w-propanol side chain supports that the existence of such reduced sidechains in the lignin structure is probable,considering the highly shielded signals in their NMR spectra, as discussed before 18,191. The formation of cornpound (E), which has eliminated an aromatic ring, may be explained i n two ways: ( a ) ring closure during hydrolysis or (b) displacement of the diarylpropanediol dur-
144
Sakakibara and Sano
+ OH
OH
OMe OMe
(m FIGURE 28 DegradationofcY,P-diarylethers (3 and aqueous dioxane at 180°C for 20 min. (From Ref. 139.)
g) by “mild
hydrolysis”using 50%
ing coupling ofradicals (Fig. 28) formed eitherin wood in situ or secondarly by homolysis of phenolic P-ethers in lignin, as shown in Fig. 29 [137,141]. As described before, the degradation products from hydrogenolysis and hydrolysis provide much important information about lignin structure and supportthe theory of lignin formation by enzymatic dehydrogenation of cinnamyl alcohols. Hydrolysis mainly cleaves the a-ethers of side chains in the lignin molecule in spite of poor model experiments, but nonphenolic P-ether cleavage occurs hardly at all [58,139]. The model experiments with p-hydroxyarylglycerol-a$-diary1 and -&aryl ethers [ 138- 1411 have indicated that homolysis occurs to a slight extent during hydrolysis, resulting in subsequent coupling of the radicals formed. But Sakakibara [l651 has stated that the formation of artificial products from protolignin by “mild hydrolysis” is negligible because of the following fact: Dehydrodiconiferyl alcohol (M)and pinoresinol and dehydrodiguaiacylpropane (106, R,=OCH,, R,=R,=H) that were found in the model experiment [138-1401 could not bedetectedeven in traces in the hydrolysatefromspruceprotolignins in spite of the proposed mechanism of compound shown in Fig. 27. The homolytic degradation of phenolic p-0-4 linkages will be summarized in the following section because of getting many informations on homolytic cleavage of phenolic P-ethers under the conditions similar to those for “mild hydrolysis” and “catalytic hydrogenolysis” of protolignins.
(e)
(m)
3. Homolysis With the aim of finding a method which would degrade lignin without involving simultaneous condensation reactions, Nimz [ 125- 1291 and Sakakibara [ 130- 1391 subjected extractive-freesoftwoodandhardwoodto“mildhydrolysis”under neutral or slightly acidic conditions followed by a percolation with hot water and a mild hydrolysis with
145
Chemistry of Lignin CH20H
CH20H
l
HCI
H A - 0 9
+
QOMe 0.
OMe
Rb
OH
0 Ra
uz&, (24.0%)
CH20H l CH II
m+RaorRb OMe 0-
OH
RC
(1) (2.6%)
OH .OMe
CHsCH-CH20H
CKOH
I
+
2xRa
CH20H H { - 0 9
FH20H j_\
OMe
Ra+Rc
-
OMe
+
H$-0 Q O M e Q O M e
Ra + Rb + RC
-
0 '
w(3.656)
polymerichydrolysisprodUCts of
FIGURE 29 Homolytic degradation of guaiacylglycerol-P-guaiacylether (g) by "mild hydrolysis" using 50% a q ~ ~ e o dioxane us (pH 3.54) at 180°C for 20 min (%: yield of the amount of starting material used). (From Ref. 140.)
146 San0
and
Sakakibara
aqueous dioxane at 1 80”C,respectively. Separately, they have isolated and identified many monolignol-to-trilignol hydrolysis products in small amounts, of which most compounds are identical to each other. The hydrolysis products due to cleavage of the benzyl aryl ether linkages have been thought to give valuable information on the end groups in lignin and the biosynthesis process of lignin, since it is probable that in the “mild hydrolysis” the hydrolytic cleavage of benzyl aryl ether linkages in lignin is the main reaction in spite of deficient experimental evidence. To obtain definitive information for the reaction mechanism of lignin under the conditions of “mild hydrolysis,” some lignin model compounds were subjected to mild hydrolysis. The hydrolysisofmodelcompounds(126,127)forphenolicandnonphenolic a$-diary1 ethers were carried out in 50% aqueous dioxane at 125-180°C for 20- 120 min [138-1411. The phenolic a-aryl ether bond in (126)was cleavaged by 41% and 83% at 140°C for 20 min and 120 min, and by 100% at 180°C for 20 min, and the nonphenolic a-aryl ether bond in by only 39% at 180°C for 20 min [139]. The latter was more resistant to mildhydrolysisthan the former. The nonphenolicP-ethercompoundwas recovered quantitatively from the reaction mixture of (g). New dimeric and trimeric compounds were obtained from the reaction mixture of (3) [138]. Guaiacylglycerol-P-guaiacyl ether was subjected to “mild hydrolysis” by two procedures, that is, 50% aqueous dioxane (pH 3.54) at 180°C for 20 min, and also water (pH 3.54) at 110°C for 48 h in place of the percolation procedures. Thin-layer chromatograms of reaction products obtained from the former were completelyidentical with those from the latter, indicating that the cleavage of the P-ether according to the two procedures proceeds by the same mechanism [140]. From the reaction mixture obtained by the former procedure of the starting material(24.0%),coniferylalcohol (1)(2.6%),pinoresinol (0.8%), 1,2-diguaiacyl1,3-propanediol (E) (1.4%), dehydrodiconiferyl alcohol (4.5%), and two trimeric compounds (1 29,130) were isolated and identified besides substantial amounts of unknown polymerizedmaterials [l401 as illustrated in Fig. 29. The compound (3.8%) was composed of phenylcoumaran and P-ether moieties, whereas (3.6%) had two P-aryl ether links. Gel filtration of the reaction mixtureshowed that their molecularweights increase with increasing reaction time, demonstrating that the degradation and polymerization of lignins take place simultaneously by “mild hydrolysis.” The polymerizationtookplaceduring the heat-up time up to 18O”C, and became predominent for 120 min to form more stabilized polylignols in large quantity. Both the relative absorbance of the “mild hydrolysis” products at A,,, about 280 nm for UV (neutral), and at A,,, about 300 nm for ionization differential spectrum ( A s i ) increase with increasing the reaction time, respectively, when measured immediately after the hydrolysis. In 348 h after the hydrolysis both of them decrease strikingly, and the absorbance at A,,,,,, about 255 nm for UV (neutral) increased reversely compared to every one when measured immediately. The UV spectrum for the reaction products, which was measured 348 h after “mild hydrolysis” of for 120 min, were very similar to that in spruce MWL except for slightly high absorbance at A 360 nm for A&,, due to phenolic conjugated carbonyl groups. The results obtained by UV analyses show that more reactive sites such as quinonemethides are present among the “mild hydrolysis” products of the model compounds, MWL, and wood-in-situ lignin [140]. When 1-guaiacyl-2-guaiacoxy- 1 -propene-3-01 (131) was subjected to mild hydrolysis with 50% aqueous dioxane at 180°C for 20 min, Hibbert’s monomers (3 1-34) were formed in addition to the starting material (15.6%) (Fig. 30). This implies that phenolic arylgly-
(m)
(m)
(e) (m)
(m),
(B)
(m)
(m)
II CH I
CHO OMe Ribkrt’s ketones
QOMe OH
(3.l-U (Total about 16%)
COOH
+ I
OH
(L31) (15.6%)
FIGURE 30 Degradation of I-guaiacyl-2-guaiacoxy- 1-propene (131)by “mild hydrolysis” using 50% aqueous dioxane (pH 3.54) at 180°C for 20 min [%: yield of the amount of (=)I. (From Ref. 140.)
148 Sano
and
Sakakibara
cerol-P-ethers in lignin are never degraded via corresponding enol-ethers under the “mild hydrolysis” conditions [ 1401. From the “mild hydrolysis” products of syringylglycerol-P-syringylether (133)by aqueous dioxane [ 14 l], syringol ( 1 4.5%), syringaldehyde (2)(1.1 YO),sinapyl aldehyde (134)( I . I %), 1-syringyl-2-syringoxy-3-hydroxypropanone-1 (136)(0.9%), D,L-syringaresinol (g) (5.6%), 2-formyl-3-hydroxymethyl- 1,4-bis-syringyl- 1,3-butadiene (3) (1.3%), and 1,2-syringyl- 1,3-propanediol (7.1 %) were isolated besides the starting material (33.3%) and polymeric compounds as shown in Fig. 3 1 . Sinapyl alcohol (2) and syringylglycerol-P-sinapylether which were not detected amongthe products, might be too thermolabile to exist in the reaction mixture, even if they were formed during the reaction process. The thermolabilities of (2,137) are apparent from the fact that they are synthesized only by reduction with LiAIH, at -30°C. The product patterns shown by “mild hydrolysis” of the two @-ether models and 134)by two procedures with aqueous dioxane at 180°C for 20 min and with water at 110°C for 48 h suggest that the reaction imitates the dehydrogenative formation of lignols and higher polymers from coniferyl alcohol and sinapyl alcohol (2). Accordingly, it is proposed that under the “mild hydrolysis” conditions phenolic arylglycerol-@aryl ether bonds may be subjected to homolytic degradation followed by polymerization as illustrated in Figs. 29 and 3 1. Phenolic @-aryl ethers as end groups in lignin lose a molecule of water to give the corresponding quinone-methides (QM), followed by homolytic cleavage of Paryl ether bonds with the formation of a p-hydroxycinnamyl alcohol and phenoxy radicals (Ra and Rb), whereas a radical transfer reaction between the former radical (Ra) and the phenolic hydroxyl groups yields a corresponding p-hydroxylcinnamyl alcohol (1, 2, or 3) and a new phenoxy radical (RC).“Endwise”addition of ap-hydroxycinnamylalcohol radical (Ra) to the latter phenoxy radical (RC)produces the trilignols in Fig. 29 and highermolecular lignols. Nimz et al. found that guaiacylglycerol-P-dihydroconiferylether gave dihydroconiferyl alcohol (41%) and dihydrodehydrodiconiferyl alcohol (phenylcoumaran, 32%), in addition to unknown products, when heated in water for 7 days [142]. Later, guaiacylglycerol-P-vanillyl ether (W)gave a phenylcoumaran coniferyl alcohol (l), vanillyl alcohol (g), and unknown condensed products as precipitates in addition to the starting material (35%) in yields of about 10, 18, 20, and 15%, respectively, when heated with water at 130°C for 4 h, and the yield of condensed products after 20 h at 130°C reachedabout30% in the absenceof starting material(Fig.32).Fromthese results Nimz concluded that a homolytic cleavage of the phenolic P-0-4 linkage occurs with water in neutral solution at 130°C [ 1431. In order to investigate the extent of homolytic reactions under the conditions of “mild hydrolysis,” Westtermark et al. [ 1441 subjected guaiacylglycerol-P-guaiacyl ether (128) and spruce wood to “mild hydrolysis” using dioxane:buffer ( I : 1) at different pH (3.69.6) and various temperatures ( I 30- 180°C). The main products obtained by the heating of spruce wood at 180°C were coniferyl alcohol (L), vanillin and coniferyl aldehyde ( 5 ) in order of peak area. The addition of a catalytic amountof FeZ+considerably increased the yield of (L) without influence on the rate of degradation. The amount of (l)formed was found to be strongly dependent on the temperatures; that is, the amount formed at 130°C was only one-fifth of that at 180°C. Its yield reached a maximum after about 100 millat 130”C, and a set of two maxima after 60 minand 120 min at 160°C as well as 180°C. then slowly decreased, showing that the coniferyl alcohol emerges from at least two different sources, and the formation and decomposition of (l)take place during the ‘‘mild hydrolysis.” The maximum amount of at 180°C exceeds the amount correspond-
(m)
(m),
”
(m
(L)
(m)
(x)
(E)
(m),
(z),
(L)
(L)
149
Chemistry of Lignin 7H20H OMe
HF-oa CHOH OMe
7H2OH OMe -H*O
0
H ? - 0 9 CH OMe
e Me0G O MOMe OH
OMe
7H20H
-6 '?H
+I[.
+M
Me0
0
0
OH
e O Q O M x e O Q O M e 0. OH
Meo60Me M e o ~ o M e
CH20H CH I
2XRa"+
HC-?H
l
I
CH2OH CH Me0O 0O M e
"t
(I4 S%)
Kb
7H2OH CH II
.CH
H+CH HC-o-kH,
Me0G O M e
FIGURE 31 Homolyticdegradation of syringylglycerol-P-syringyl ether (133)by "mild hydrolysis" using 50% aqueous dioxane (pH 3.54) at 180°C for 20 min (%: yield of the amount of (g)]. (From Ref. 141.)
150
Sakakibara and San0
...goMe CH
YH20H CH qH2OH
Ra+Rc
H-C
L 1
Q
CHo OMe
Me0
Ra+Rb
c-c
$H I
-
$oM;o Me0 OH
+ I I,O
Me0
OMe
0
Me0 OH U)(7 1%)
FIGURE 31
Continued
ing to the total content of coniferyl alcohol end groups (about 2%) in softwood lignin. This means that a considerable part of the coniferyl alcohol must originate from sources other than a-ether end group substructures in lignin. The stability of coniferyl alcohol (1) toward “mild hydrolysis” in 50% dioxane (pH 7) at 130°C demonstrated that coniferyl alcohol is degraded or polymerized fairly rapidly even at 130°C. And guaiacylglycerol-Pguaiacyl ether ( 128), which was degraded by 80% in the same medium after 40 min at 1 8O”C, a f f o r d e d 0 at a 20% mole yield. No Hibbert’s ketones (31-34) could be detected in the reaction mixtures even when about 50% of ( 128) was degraded in 50% dioxane at a pH as low as 2.7 and 160”C, indicating that a c i d o 5 i s does not occur by “mild hydrolysis.” Based on the above results, Lundquist et al. [ 1441 concluded that the use of “mild hydrolysis”asa tool in lignin analysis leads to erroneous and confusing results if the homolytic cleavage of the @-ethers is neglected. It is well-known that phenolic P-ethers in lignin are prone to undergo reactions via ionic intermediates under acidic and basic conditions. However, it has been reported recently that the P-etherbond i n syringylglycerol-P-syringylether (133)is subjected to homolysis under conditions similar to those in a soda cook [ 1451. Furthermore, Sipila et al.[l461 allowed syringylglycerol-P-syringylether to stand in aqueousdioxane solutions at pHof 4-7 at roomtemperatureandfoundsyringaresinol (G),P-l (E: R,=R2=OCH,) and 2,6-dimethoxy-p-quinones, giving further evidence for the existence of homolytic P-aryl ether cleavage in delignification of hardwoods. Sano [ 147,1481 subjected extractive-free oak wood meal, guaiacylglycerol-P-guaiacy1 ether and its 4-0-methyl ether to “solvolysis” in p-cresol-water ( 1 : 1 ) at 180°C for 30 min in order to explain the delignification mechanism of wood lignin by solvolysis pulping with aqueous phenol at elevated temperatures. Fromreaction products of the wood, six compounds (143-148) were isolated and identified, as the same cresolated compounds
(m)
(m),
151
Chemistry of Lignin
KMe OMe
+
Q O M e
OH
20 h
OH
OH
+
W (35%)
condensed products (30%)
FIGURE 32 Degradation of phenolic P-ethers (3 and 141)by “mild hydrolysis” with H 2 0 at 100°C or 130°C (%: yield of the amount of (139)or (E)]. (From Ref. 142.)
with guaiacyl and syringyl rings also obtained, respectively, from the reaction products of guaiacylglycerol-P-guaiacyl ether (128)and sinapyl alcohol (2) treated under the same conditions. The reaction mechanism by phenolysis has been illustrated asfollows(Fig. 33). The cleavage of phenolic @-ethers in lignin proceeds via homolysis to form two freeradicals, which are trapped by the phenols as a solvent and/or other active intermediates to give p-cinnamyl alcohols (1-3) from end groups and new phenol groups in lignin. The latter are further cleavaged in reaction sequences of the “peeling” type to lead the extensivedepolymerization of lignin.p-Hydroxycinnamylalcohols (1-3) aredehydrated to extended quinonemethides (E), which are condensed with the phenols by ionic reactions. The resulting resonance-stabilized phenolated compound are oxidized with the phenol radicals and/or lignin radicals to the corresponding radicals, followed by radical coupling. Interestingly, it may be noted that no syringaresinol (G)was detected among the solvolysis products of oak wood in spite of the inactive compound toward the solvolysis reaction [ 147,1481. Lin et al. [ 1501 recently reported that is subjected to homolysis under conditions for the liquefaction of wood with phenol at elevated temperatures. Thus, homolytic cleavages of phenolic P-arylethers in wood lignin can occur at elevated temperatures in many technical processes, for example, high-yield pulping and steam hydrolysis [ 1491, and in thedegradationproceduresfor structural studies under
(m)
(m)
152 San0
and
Sakakibara
coupling Radical coupling Radical Products
Products
W
FIGURE 33 Homolytic degradation of (3) by “solvolysis” using p-creso1:water:acetic acid (9: 1:O.l) at 180°C for 2 h. (From Ref. 147.)
neutral conditions at pH 2-9 and elevated temperatures, for example, mild hydrolysis and hydrogenolysis to yield p-hydroxycinnamyl alcohols and their radicals, and end phenoxy1 radicals in lignin, followed by formation of condensed polymers and chromophores, which influence the brightness and brightness stability of wood and high-yield pulps, and organosolv pulpings. The mild catalytic hydrogenolysis of protolignins has been studied extensively to obtain structural information. Sakakibara et al. [99-1171 subjected protolignins to catalytic hydrogenolysis in 60-90% dioxane containing a catalyst, copper chromium oxide,at 220240°C for 1 h. The hydrogenolysis of protolignins appears to proceed as follows: protolignins are depolymerized and solubilized in aqueous dioxane at 220-240°C higher than those for “mild hydrolysis,” then subjected to catalytic hydrogenation and hydrogenolysis to form “stabilized” hydrogenolysis products. The reaction mechanism for the solubilization and hydrogenolysis of protolignin needs clarification in details to apply the catalytic hydrogenolysis as a meaningful tool in the elucidation of lignin structures. On treatment of 1,l-diphenyl-2-picrylhydrazinewith aqueous dioxane at 180°C for 30 min, the hydrazyl radical is formed in large amounts, but not at below 140°C [ 1381, indicating that phenolic hydroxyl groups may be converted to phenoxy radicals at elevated temperatures.
153
Chemistry of Lignin
OH
-
CH II
OMe
’
O O C H 3 0
FIGURE 33 Continued
D. Acidolysis, Thioacetolysis, and Thioacidolysis
1. Acidolysis with 90% Aqueous Dioxane Containing HCl Since it had been found that refluxing of wood with 90% aqueous dioxane containing 0.2 M HCI, results in the formation of an ether-soluble oil in addition to a high-molecular lignin product, this treatment, “acidolysis,” was subsequently applied both to model compounds and to lignin preparations instead of ethanlysis. Upon 4 h acidolysis of guaiacylglycerol-P-guaiacyl ether (g), the P-ether linkage was cleaved, guaiacol being released, and furthermore, m-hydroxyl-guaiacylacetone (31) could be isolated in a yield of 53%. The latter was slowly further converted, yielding t h e isomeric ketols (3 1,32, I5 1 total yield: 15%), as well as small amounts of ketones in addition to only 3 S % of unchanged starting material as shown in Fig. 20 [IS l]. The acidolytic cleavage of the P-ether linkage in (128)is assumed to proceed via a benzylium ion and an enol ether (E), which is susceptible to acid hydrolysis, followed by formation of monolignols (Hibbert’s ketones 3 1 -34,15 1 ) with carbonyl groups. When spruce Bjokman lignin (MWL) was subjected to the acidolysis treatment under the same conditions, the low-molecular portion of the resulting mixture could be resolved by gel filtration into fractions containing monomeric. dimeric, and oligomeric compounds, respectively. As shown in Fig. 34, in the monolneric fraction the same ketones a s those
(e)
(2,s)
Sakakibara and Sano
154
HCO
l
y
2
H
+
+C,
um
Q O M e
0
I
OH
OH W
1
CH20H I
CH3 I
CH3
I
CH3
CH3
F="
c=o
6. 6 6 6 6 c=o
c=o l
-
1
I
I
I
H OH
OMe OH
OMe
' OMe
OH 0
U
m
0
CH20H
HCO
HS;0
c=o
HC
HC
I
I
66 I
1l
OH
OH
uiz,
0
W
II
OH 0
FIGURE 34 Monomeric products obtained by acidolysis of spruce MWL. (From Ref. 124.)
formed from model compounds (128) were detected, the predominating ketol (31)being obtained in yields of S-6% of the lignin. In addition, the presence of small amounts of homovanillin and formaldehyde (E) was demonstrated. The side reaction can be regarded as areverse Prins reaction of the benzyliumion intermediate. Theseresults constitute clear evidence of the substructures of the guaiacylglycerol-P-aryl ether type. The monomer fraction contained small amounts of ketol coniferyl aldehyde Q), and p-coumaraldehyde (E). In a similar monomeric fraction obtained from the acidolysis of birch MWL, a number of syringyl analogs were detected in addition to most of the compounds shown in Fig. 34 [ 1521. The yields of the syringyl monomers were higher than those of the guaiacylmonomers, although the ratio of syringyVguaiacyl is about 1 : 1 in birch. This is due to the fact that some of the guaiacyl units are linked to an adjacent unit by S - S , p-S, and S-0-4 bonds. which cannot occur in syringyl units. From the dimeric fraction obtainedfromspruce lignin, compounds (45,154- 160) were isolated and identified as summarized in Fig. 35. With the exception of trace constituents ( l S5,160), the dimeric fraction of birch lignin gave the same guaiacyl compounds,
(x)
(m),
"
CHpOH
CHpOH I c=0
I
c=o I
?H
?"
I
qH2
H3C,
+HC OM II.
Ff +OMe
6 GOMe
7-0
OH OMe
QOMe OH
OH
OH
ui8)
OH
(m)
HC-CH3
I
OMe
(rn)
0
'CH2
'
HpC' HCI
Me0
w
UIZ)
AH I
0 OH
Q O M e OH
(m
HC-YH I HpC-, /CH O I
(41,
Me0Q O M e OH
FIGURE 35 Dimeric products obtained by acidolysis of spruce MWL. (From Ref. 124.)
OH u.33
156
Sakakibara and San0
the corresponding syringyl analogs with one or two syringyl nuclei, and, furthermore, the stereoisomeric compounds D,L-syringaresinol ( S ) and D,L-epi-syringaresinol (E). The phenylcoumarone (154)and the stilbene (155)originate from a lignin substructure as shown in Fig. 36. The phenylcoumarone (%), which is formed in much higher yield than the latter, has a characteristic and very strong UV absorption 11531. This permitted its quantitative estimation, which indicated that about 10% of the C, units in the spruce lignin are connected to anadjacent unit byan a-0-4 aswellas a p-5 linkage, giving rise to a phenylcoumaran system. The acidolytic conversion of a hydroxylmethylsubstituted phenykoumdraninto a methyl-substitutedphenylcoumarone is readily explained by a sequence of ring opening, allylic rearrangement, and recyclization. The dimeric compounds (156-159)all exhibit only one side chain per two guaiacyl residues. It was postulated that these compounds could arise from a 1,2-diguaiacyl-1,3propanediol substructure (E)incorporated into lignin by acid-hydrolyzable linkages (Fig. 37). A plausible mechanism for their formation has been presented [ 1541. Compound (E) and related compoundscarryingone or twosyringyl nuclei were isolated from“mild hydrolysis” products of softwood and hardwood, respectively, [89,129,133,134], and (3) was also detected among the low-molecular productsof coniferyl alcohol dehydrogenation. The biogenesis of the lignin substructure (E)can be visualized as shown in Fig. 21. A p-l coupling between a coniferyl alcohol radical and the radical of a p-hydroxybenzyl alcohol end group forms (E)and a glyceraldehyde-2-aryl ether group Experimental evidence for the presence of glyceraldehyde end groups of type ( 4 0 ) was provided by the detection of pyruvaldehyde (150,methylglyoxal) in the acidolysis mixtures from spruce and birch MWL. The mechanism of the acidolytic formation of pyruvaldehyde is presented in Fig. 38. Colorimetric determination of the aldehyde formed on acidolysis of spruce and birch MWL, as well as of model compounds (g), indicated that only about 2% of the C, units of lignin were bound to glyceraldehyde as shown by formula (S). The results of ‘H-NMR studies on the aldehyde groups present in spruce MWL point to a similar value for the amount of glyceraldehyde groups. This figure, however, appears very low in view of the fair yields of degradation products of the p-1 type obtained by thioacetolysis of
(c).
s? r 6
2. a
a
L
Q O M e OH
w
OH (1121
acidolysis
Y O M e OH
w
(From Ref. 154.) 1,3-diolunits (2). FIGURE 37 Acidolysis of 1,2-diarylpropane-
m
I
Sakakibara andSan0
158
c-c-c
FIGURE 38 Acidolysis of glyceraldehyde-2-aryl ether units
(S).(From Ref. 90.)
beech wood. It has been proposed by Sarkanen that the unconjugated carbonyl groups in spruceMWL,whichamount to about 10 carbonylgroupsper 1 0 0 C, units, mightbe regarded as being present in glyceraldehyde groups. This proposal, however, does notfind support in the analytical results mentioned above. In Fig. 39, the substructures which have been disclosed by the acidolysis procedure are summarized. Of these structures, the arylglycerol-P-aryl ether structure undoubtedly is the most abundant one. As already mentioned, C, units which are linked to an adjacent unit by forming a phenylcoumaran system occur in spruce lignin in an amount of about 10%.D,L-syringaresinol ( g )and its stereoisomer D,L-episyringaresinol have also been found among the acidolysis products from birch. The corresponding guaiacyl compounds (S), however, could not be found in spruce or birch acidolysis mixtures. If pinoresinol (44) structures are present in lignin in
(m)
t; C,
C
c:
0’
C
I G O M e H2COH HC-0
MeoQoMe H,C*O-?H
Chemistry of Lignin
159
appreciable amounts, one must assume that they are linked to adjacent units by acid-stable bonds, i,e, 5-5 and 5-0-4 bonds, to an unexpectedly great extent. The "NMR spectrum of spruce lignin also indicates a very low content of pinoresinol structures. However, experimental evidence in favor of the occurrence of such structures in conifer lignin has been presented. A further acidolysis product exhibiting coupling, namely, D,L-divanillyltetrahydrofuran (E), was isolated in small amounts from spruce lignin acidolysis. The compound differs from the other dimeric acidolysis products in possessing a lower degree of oxidation. Degradation of beech wood by thioacidolysis afforded the syringyl analog. Its formation seems to involve an oxido-reduction process, but it remains open what substructures (@) in lignins originated from [154].
(e)
2. Thioacetolysis and Thioacidolysis Thioacidolysis causes cleavage of P-0-4 bonds, and brings a more deep-ground fragmentation of the lignin than acidolysis [95,155]. As much as 91% of the lignin of beech wood and 77% of the lignin of spruce wood were degraded to mixtures of monomeric to tetrameric products. The principle of the three-step degradation method has been formulated by Nimz as shown in Fig. 40. Treatment of wood with thioacetic acid and boron trifluoride converts the arylglycerol-P-aryl ether unit (40.1) via the benzylium ion ( 4 0 . 2 ) into the Sbenzyl thioacetate (=). Subsequent saponification with 2 N NaOH at 60°C gives a benzyl thiolate ion (40.4) which loses the P-aryloxy group by nucleophilic attack of the neighboring thiolate ion on the P-carbon atom to give an episulfide The latter dimerizes to dithianes or polymerizes to thioethers. In a final step, treatment with Raney nickel and alkali at 115°C removes the sulfur and yields the reduced phenolic reaction products. The 20 dimers obtained from beech wood are shown in Fig. 41. Most of the bond typesexhibited by these dimers are identical withthoserevealed by otherdegradation
(a).
cn,on l
I
I HCOAr 13 F,
R'
CH20COCHs
CHPOH
HCOAr Cl I$X)SI I
NaOl I
OMe
R'
OR (40.2)
OR (4.3)
CHZOH
CH2R
l
I
HqSo
R'
OMe OH
OH R=H or OMe K'=llorOlI (40.7)
FIGURE 40 Degradation of lignin by thioacetolysis with thioacetic acid.
(From Ref. 95.)
160
Sakakibara and San0
&Q'16 OH
R
OMe OH
H $ oOH O M e
R OMe / OMe OH
R=H or OMe
OH R=H or OMe
CH3
CH3
HC
I
Me0
OMeMeO OMe OH OH
OH
R
OMe Me0
OMe
OH
\
R=H or OMe , R'=H2or =O
/
u6i, (0.5%)
CH3
I
CH3
I
C
Me0
OMe
R
OHOH R=H R=OMe or OH
c166)(0.45%)
FIGURE41 95.)
R=OCH3.
R=OMe (142) (0.4%)
OH
OH R=H or OH
(0.1%)
0 (0.3%)
Dilignols obtained from beech protolignin by thioacetolysis (% of lignin). (From Ref.
Chemistry of Lignin
161
methods, especially acidolysis and oxidative degradation cited above. The a-p-junction (165) found in some compounds (0.5%) was assumed by Nimz and Das [95] to be present i n e e c h lignin, although it cannot be the result of a dehydrogenation. Its formation and that of some related structures is assumed to be due to a proton-catalyzed polymerization of coniferyl alcohol (1)or coniferyl alcohol end groups caused by the natural acidity of the cell sap. However, we must also point to the possibility mentioned by Nimz [ 1801 that (1)andsinapylalcohol (2) may arise during the degradation process, analogous to the formation of (L) as an intermediate in kraft cooking of spruce lignin. The heating with alkali in the last degradation step may cause Michael-type additions of the p-C atom of coniferyl alcohol to the a-position of quinonemethide structures whichalsocanbe assumed to be intermediates. The a-p-linked products may accordingly be artifacts. On the basis of the yields of crude and pure degradation products, Nimz has calculated the frequencies of the various bond types in beech lignin and has also proposed a structural scheme for this lignin (Fig. 46). Recently,a new acid degradationmethod, thioacidolysis (solvolysis in dioxaneethanethiol with boron trifluoride etherate) has been studied by means of a reproducible and mild routine procedure to obtain detailed structural information about lignin [ 1561591. The acid degradation of lignin was composed of two consecutive thioacidolysis and desulfuration of thioacidolysis products over Raney nickel as illustrated in Fig. 42, which is similar in principle to that proposed for thioacetolysis (Fig. 40). However, thioacidolysis is carried out using a few milligrams of sample in dioxane at 100°C for 4 h instead of thioacetolysis performed at 20°C for 1 week. Reaction conditions for the former seem to be more advantageous as a tool for structural studies of lignin than those for the latter. The thioethylated monolignols and the desulfurated dilignols of spruce MWL and wood are shown in Fig. 38 [1591. Among the thioethylated monomers from spruce MWL, the compounds (170,171), whichwereformedfromuncondensed p - 0 - 4 linked units, were obtained in a total yield of 9 3 % of the monolignols. They reflect the higher content of uncondensed p - 0 - 4 linkages in the MWL products and from coniferyl alcohol end groups were obtained in a total yield of 6.6% based on the monomers. The compounds and orginating from coniferyl aldehyde end groups and from dihydroconiferyl alcoholendgroups, respectively, weredetected in trace amounts.The yields of main dilignols obtained from spruce MWL and wood are shown in Fig. 43 and characterize the various types of condensed linkages in softwood lignin. From their yields, it can be concluded that p-S, 5-5, and p-1 linkages are present as major types of condensed interunit linkages in softwood lignin. In addition, the dimerswithdiphenylether (181)(4-0-S), phenylisocoumaran (p-5), and tetrahydrofuran (M)(p-p) structures, of which the structures were assigned only from their fragmentation patterns, were detected in trace amounts, and their linkages seem to be minor types among condensed linkages. However, the latter two dilignols have been assigned to be compounds with different structures in two papers reported by the same authors [ 159.1, indicating that they need to be isolated and identified. The total area of GC peaks due to the dilignols assigned accounts for more than 90% of all the peaks corresponding to dilignols in the chromatograms of spruce MWL and spruce protolignin. The total amount of the dilignols is about 30 mole% of the main thioacidolysis monomers obtained from both of the lignins. The relative importance of condensed interunit linkagesimplied by the mole ratio of the thioacidolysis dilignols is almostequal between spruce MWL and sprucewood lignin in situ. The yields of compounds which were characterized as monolignolsanddilignols among the thioacidolysis mixture were only 40-S0% of lignin [ 1593, which may reflect the limitation of thioacidolysis results to the degradable part of lignin.
(m)
(m) (m)
(m) (m),
162 San0
and
Sakakibara
H2COH HCSEt
I l
H2yH HCORp
HCOR2 HCOR2
I
@,R1
F 6
BF3 E(SH
_ I )
OMe
OR
H2COH
OMe9F3
H2COH
OR
I
I
COR2
H27OH
OH
HpCOH
-
I
I
6z; 6E":;61 OR
It
OH
!$p
I I
'OMe OR
H
OR
OR
OR
OH
OH
FIGURE 42 Reaction mechanism of p-0-4 substructure units by thioacidolysis and subsequently desulfuration with Raney nickel. (From Ref. 156.)
In order to use the interesting thioacidolysis method as a routine procedure for the characterization of the total structure of lignins, it is necessary that the thioacidolysis productscontaining trilignols to oligolignols be clearly characterizedandacid-derived condensation by thioacidolysis clarified.
V.
STRUCTURAL MODELS FOR LIGNINS
A.
Frequencies of Functional Groups and Typical Linkage Types in Lignins
Summarized in Fig. 44 are the main types of lignin structural units which were obtained from the various lignin degradation products described above. Frequencies of the functional groups and the typical linkage units in spruce and birchMWL, and beech protolignin are collected in Tables 10 and 11, respectively. The most important linkage types in the lignin molecule are p-0-4(B) and then p-5 (g),5-5 (E), p-1 (C), and a-0-4 (A). The pp linked units are represented by pinoresinol (g), syringaresinol (g), and dibenzyltetrahydrofurans F(c) (160 and Pinoresinol substructure (@-p)may be rather minor in softwood lignin, but syringaresinol (45) - is abundant in hardwood lignin. Though the com-
x).
Me
dsEt do"
Chemistry of Lignin
&Et
OMe
Et$
SEt Et$EtS
163
SEt
OMe
OH OH
OH
0
0
OH OH
OH
uze,
0
uz2,
W
R
Me0
OMe OH
5-5 series
p1 series
4-0-3 series
Meor i
H0
Me0
H O H z C e Me
R2
\
p5OH \ / series OMe OH
OMe HOH2CfMe p3OH \ senes
p5 series
CH3 R=H.
p5 senes
or CH20H
u8L,
OMe
OH
p p series
Rl=CH3 or CH20H R2=H 01 CH3
u&+M=33%)
FIGURE 43 ThioethylatedmonomersandRaneynickel-desulfurateddimersobtainedbythioacidolysis of spruce MWL (% of dimers). (From Ref. 158.)
(M)
pound was obtained as one of the important substructures next to A, B, C, D, and E typesfromacidolysisand thioacidolysis products of spruce MWL, it remainsopen whether is a substructure in lignin or acid-condensation products of (101:R=OH). P-Aryloxyglyceraldehyde units B(a) have been estimated by acidolysis and 'H-NMR. 40-5-Diphenyl ether and 0-6 units have been confirmed by not only oxidation but also catalytic hydrogenolysis. By the latter, frequencies of bond types has not been estimated. The yields of oxidation products were used in the estimation of the bond types in the MWLs, though certain assumptions, e.g., regarding the actual and theoretical yields of oxidation products, are involved [ 1611. Naturally, the frequency values in Tables 10 and
(m)
164
Sakakibara and San0
F
8-Q
E - 0 - 0 I
6" 6
6
C
A
B
"8 F'
go
F F
C-
FC
l
I
F
E
F
I
?
C I
D
F C?-
C
FC
F
cI
$
I
C
G
H
0 G(traces)
F F
FC
6-6 I
I
FIGURE 44 Typical linkageunitsin
lignin.
11 are to be regarded as approximate rather than accurate, although mostofthem are fairly reproducible. Some uncertainty is attached to the values (0.02-0.15) given for bond type C in spruce MWL in spite of differing estimation methods. Sarkanen [ 1721 has stated that p-1 units are main substructures in endwise lignin for the middlelamellaregion rather than in bulk lignin for the cell wall. However, Lapierre et al. [l581 have reported that p-
Chemistry of Lignin
165
TABLE 10 Functional Group and Structural Unit of Spruce
MWL
Functional Groups units
Functional groups and structural Aliphatic OH 168,701 Phenolic OH [82,701 Total carbonyl
0.93 0.33
c,,=o
Unconjugated C=O Ar-CH=CH=CHO Ar-CH=CH-CH20H Phenolic C,-OH Nonphenolic C,-OH
C&
References
1.09, 0.26, 0.20 0.06-0.07 0.10 0.03-0.04
1591 [S91 1591 1411
0.03
1441
0.05-0.06 0.15, 0.10
176.781 [59,781
~~
A: a-0-4 (open)
Phenolic Nonphenolic B: p - 0 - 4
c: p-5 Noncyclic D: p-l E: 5-5, 5-6 F: p-B
Pinoresinol units G: 4-0-5, 4-0-1
0.12, 0.07, 0.06-0.08 0.04, 0.02 0.05-0.09, 0.06 0.49-0.5 1, 0.50 (0.25-0.30, 0.3-0.5)'' 0.02b 0.14, 0.9-0.12 0.03 0.15, 0.02, 0.07 0.19-0.22, 0.10-0.1 1 0.13 0.05- 1 .O, 0.02-0.03 0.07-0.08, traces
"Except displaced side-chain unlts. "Arylglyceraldehyde-P-arylether. Source: Ref. 167.
1 units are almost as frequent as in spruce in-situ lignin and basis of the results obtained by thioacidolysis.
MWL preparations on the
B. Structural Models for Softwood Freudenberg [ 1631 attempted to constructa structural formula for softwood lignin, utilizing theknowledgeobtainedfromtheenzymaticdehydrogenation of coniferylalcohol. The formula, which was composed of 18 units, was later modified several times 1164- 1661. Adler [ 1671 has collected theprominent substructures of spruce ligninin a structural model comprising 16 C& units. Glasser [ 1681 has proposed a structuralmodelbasedon 81 phenylpropane units that was constructed by computer simulation. A structural model of softwood lignin consisting of 28 units was proposed by Sakakibara [ 1691 as shown in Fig. 45. Alternative units are indicated in brackets against letter (b). The linkage patterns between thephenylpropaneunitsarebased mainly on results obtained by hydrolysis and hydrogenolysis. The formula of the models for spruce lignin are calculated as C,H,,,~,O2,,,(OCH,),,,,, which agrees well with those of spruce MWL shown in Table 4. The formula is a tentative one and is constructed only from information obtained so far, omittingunits,theexistence of which isat present uncertain.Onlypart of theactual
and Sano
166 TABLE 11
StructuralUnits(per
1 0 0 C&, units) of Birch MWL and Beech Lignin
Beech [95]
Birch [ 1671 Units A: a-0-4 (open) B: p - 0 - 4 34-39
Total
G
S
6 60 2 7
22-28
p-0-4"
c: p-l D: p-5 E: 5-5 F: P-p
Total
6 4.5
2.3
4.5 3
P-B p-P and L Y - ~ ~ G: 4-0-5, 4-0-1 H: C(a)-2, C(a)-6 I: a-P
1 1-1.5
5.5 0.5- 1
6.5 1 .5-2.5
65b
15 6
5 2 0.5 1.5
2.5
"In glyceraldehyde-P-aryl ether. hA + B. 'In dibenzyltetrahydrofuran units. 'In tetralin units.
number of these units has been arbitrarily selected because of the lack of adequate quantitative data.
C. Structural Models for Hardwood Lignin Nimz [l701 proposed a constitutional scheme for beech lignin on the basis of the results from mild hydrolysis and thioacetic acid degradation of beech lignin (Fig. 46). This structural model consists of 25 phenylpropane units containing 14 guaiacyl, 10 syringyl, and one p-hydroxyphenyl moiety, of which six units can to some extent be replaced by the dilignol units enclosed in the brackets. The models give a representative section from a beech lignin molecule 10-20 times larger, in which the 10 different bond types are randomly distributed. Glyceraldehyde-2-aryl ether units B (a) are not detected on degradation of beech lignin, but their presence is evidenced as a counterpart by the occurrence of p1 dilignol units (C) as shown in Fig. 21. The formula of this structural model is calculated as C,H,,,,O,,,(OCH,),,,,, which is close to the formula shown in Fig. 4. Furthermore, the I3CNMR spectrum calculated for the proposed structure was compared with that observed for beech lignin.
D. Heterogeneity of Protolignin These structural modelsareonlyaverage pictures for lignin structures that may have different chemical configurations in the different morphological regions of the cell wall. Fergus and Goring [ 17 I ] indicated varying amounts ofsyringyl- and guaiacylpropaneunits in the various cell wall layers and middle lamella of birch wood by means of UV spectrophotometry. Matsukura et al. [ 1721 showed by oxidation and alcoholysis of spruce wood that the lignin polymer has a heterogeneous structure. Furthermore, it has been pointed out that lignin in the middle lamella region may possess more of the nature of an endwise
167
Chemistry of Lignin
H$?-0“
bH W O M e
FHOH FHOH CH20HI
FIGURE 45 A structure model for softwood lignin.
CH20H
168
Sakakibara and San0
7HpOH HV-
-0
OMe Me0 MeO MeO
MeO
OMe
OMe
Me0 OMe Me0 MeO
OMe -0
FIGURE 46
0-
-0
OH
A structure model for beechwood lignin. (From Ref. 170.)
polymer than that permeating the polysaccharide matrix in the S2 layer [ 1731. Compression wood contains not only more lignin but also more condensed-type units than normal wood lignin [21]. The reason may be explained by the fact that the outer S, layer of compression wood is highly lignified, whereas the middle lamella is not completely lignified [ 1741. The controversysurroundinglignin-carbohydratecomplexes(LCC)hasbeendebated for a long time. In spite of numerous studies, the question of whether the association between lignin andcarbohydrates is physicalorchemical in naturehas not yetbeen resolved. However, the evidence for chemicalbondsbetweenthemhasbeengrowing gradually. For instance, enzymatic hydrolysis of LCC preparations gives concentrated LCC
Chemistry of Lignin
169
fractions that indicate the existence of covalent bonds between lignin and carbohydrates, because enzymes do not cleave lignin-carbohydrate linkages [ 175- 1801. The structure of protolignin must take into consideration the presence of LCC linkages. Some typical forms of LCC linkages have been suggestedby Freudenberg et al., who isolated phenylpropanecane sugar compounds from the mixture arising from the simultaneous enzymatic dehydrogenation of coniferyl alcohol and cane sugar [ 181, l 821. Finally, a word should be mentioned about Brauns lignin (BL), which Brauns [ 1831 first isolated from black spruce by extraction with ethanol in 1939. Since then, BL has been consideredto be natural lignin and has been used for several basic studies of lignin. However, it is not clear whether BL is a true lignin or not, as Freudenberg [ 1841 pointed out that BL may be a fraction of resinous material. Recently, various new lignans have been isolated [ 1601. They consist of dimeric, trimeric, and tetrameric phenylpropanes that are very similar to the lignols from degradation product mixtures, as already mentioned, except for optical activity and some other details. The existence of monomeric, oligomeric, and polymeric phenylpropanes in the lignan fraction suggests that these constitute a continuous spectrum of lignans. In conclusion, BL can be considered a polymeric fraction of lignans and not a true lignin.
VI.
OUTLOOK
The concept of lignin as dehydrogenation polymer of p-hydroxycinnamylalcohols is now well established. The efforts to clarity the structures of the different types of lignin have resulted in a detailed picture of the various modes in which the C& units are linked together in the lignin polymer. Whereas there is good agreement regarding the frequency of the predominant type of linkage, that is, arylglycerol-p-aryl ether substructures, there is even now some uncertainty regarding the proportions of some linkage units, such as noncyclic cy-aryl ether (A), p-! (C), @-p(E), andothersoccurring in minoramounts. “Mild hydrolysis” and “catalytic hydrogenolysis,” which has been used as the conventional degradation methods to characterize the structures of protolignin, appear to lead to erroneous and confusing results by homolytic cleavage of phenolic @-aryl ether linkages and subsequent secondaryradical couplings, so the elucidation of their reaction mechanism of protolignin will be required. Acid-catalyzed degradation, such as acidolysis and thioacidolysis, which give rise to self-condensation of lignin, will deviate to a certain degree froma useful tool toanalyze total linkages of phenylpropane units in lignin. We will require much continued effort to analyze total linkage units in at least MWL and also unchanged lignin in wood. Lignin, which is the most abundant natural polymer next to cellulose, is produced toabout 80 milliontonsandburnedtorecoverkraft-pulpingchemicalsandtomake energies for pulping and papermaking. Regenerated wood biomass will have to be applied to the saving andor substitution of petroleum oil for both energy and chemicals in the future for the sustainable development of the world without environmental pollution. Although wood cellulose is the most predominant pulp material, it will be utilized together with other polysaccharides and old paper as raw materials for about 95% of petrochemicals. The polysaccharides may be converted easily to various chemicals, but the immense problem of finding industrial applications for lignin remains a great challenge to wood chemists. Continued efforts will be required to finish the conversion of wood biomass, that is, wood biomass is separated into pulp, hemicellulosic sugars, lignin, and extractives
170 San0
by a novel process with less amounts wood chemicals of high value.
and
of energy and environmental
Sakakibara
pollution to use as
REFERENCES T. Terashima, in Chemistry of Lignin (J. Nakano, ed.), Yumi Publishers, Tokyo, p. 70 (1978) (in Japanese). 2.G.Aulin-Erdtman, Svensk Pupperstidn., 55:745-749(1952). 3.G.Aulin-Erdtman, SvenslcPapperstidn., 56:91-101(1953). 4.G.Aulin-ErdtmanandL.Heghom, Svensk Puppersridn., 60:671-681(1957). 5. G. Aulin-Erdtman and R. Sanden, Acra Chem. Scand., 22: 1187- 1209 (1968). 6. J. C.Pew, J . Org. Chem., 28:1048-1054(1963). 7.J.C.Pew, Nature. 193:250-252(1962). 8. 0. Goldschmid, Anal. Chem., 26:1421-1423(1954). 9. E. Adler and K. Lundquist, Actu Chem. Scand., 17: 13-26 (1963). 10.A.G.SchdningandC.Johansson, SvenskPupperstidn., 68:607-613(1965). 11.G.Wegener,M.Przyklenk,andD.Fengel, Holdorsch., 37303-307 (1983). 12. H. L. Hergert, in Lignins (K. V. Sarkanen and C. H. Ludwid, eds.), Wiley-Interscience, New York, pp. 267-297 (1971). 13. S. Kolboeand 0.Ellefsen, Tuppi, 45:163-166(1962). 14.K.V. Sarkanen,H.-M.Chang,andB.Ericsson, Tuppi, 50572-575 (1967). 15. V. Sarkanen, H.-M. Chang, and G. G. Allan, Tuppi, 50583-587 (1967). 16. K. V. Sarkanen, H.-M. Chang, and G.G. Allan, Tappi, 50587-590 (1967). 17. C . H. Ludwig, B. J. Nist, and J. L. McCarthy, J. Am. Chem. Soc., 80:1186-l196 (1964). 18. C. H. Ludwig, B. J. Nist, and J. L. McCarthy, J. Am. Chem. Soc., 8 0 1 196- 1202 ( 1964). 19. B. L.Lenz, Tuppi, 51511-519(1968). 20. D. E.Blandand S. Sternhell, Ausrral. J . Chern., 18:401-410(1965). 21.N.MorohoshiandA.Sakakibara, Mokuzui Gakkaishi, 17:393-399(1971). 22. K. Horisaki, K. Shimatani, Y. Sano, and T. Sasaya, in 37th Lignin Symp., Kyoto, Japan, pp. 125- 128 (1992). 23. K. Lundquistand T. Olsson, Acrn Chem. Scond., B31:788-792(1977). 24. K. Lundquist, Actu Chem. Scand., B33:27-30(1979). 25.K.Lundquist, Actu Chem. Scand., B34:21-26(1980). 26. K. Lundquist, A. Paterson, and L. Ramsey, Acta Chem. Scand., B37:734-736(1983). 27. S. LiandK.Lundquist, Nord. Pulp Paper Res. J., 9:191-195 (1994). 28. R. M.Ede,G.Brunow,L.K.Simola,and J. Lemmetyinen, Holdorsch., 44:95-101(1990). 29.H.-D.LtidemannandH.Nimz, Mulcrornol. Chem., 175:2409-2422 (1974). 30.H.Nimz, I. Mogharab,andH.-D.Ltidemann, Makromol.Chern., 175:2563-2575(1974). 31. H.NimzandH.-D.Ltidemann, Hol$orsch., 30:33-40(1976). 32.D.GaganireandD.Robert, Makromol.Chem., 178:1477-1495(1977). 33. J. R. ObstandJ.Ralph, Holdorsch., 37297-302 (1983). 34.C.Lapien-eandB.Monties, Holdorsch., 39:367-368(1985). 35.A.Bjdrkmanand B . Person, Svensk Pupperstidn., 60:158-169(1957). 36. K. Freudenberg and A. C. Neish, in Molecular Biochemistry and Biophysics, Vol. 2, SpringerVerlag,Berlin-Heidelberg,p.113(1968). 37. D. Fengel,G.Wegener,and J. Feckel, Holdorsch., 3551-57 (1981). 38.H.Nimz, Holgorsch., 20:105-109(1966). 39.A.Sakakibara, Rec. Adv. Phytochem., 11:117-139(1977). 40. E. Adler,K.J.Bjorkvist,and S. Haggroth, Acta Chem. Scund., 293-94 (1948). 41. E. AdlerandL. R. Ellmer, Acra Chem. Scand., 2339-840 (1948). 42. E. Adlerand J. Marton, ActaChem. Scand., 15:357-369(1961). 43. J. Martonand E. Adler, Acra Chem. Scand., 15:370-383(1961). 1.
Chemistry of Lignin 44. 45. 46. 47. 48. 49.
50. 5I. 52. 53. 54.
55. 56. 57.
58. 59. 60. 61. 62. 63. 64. 65. 66. 67. 68. 69. 70. 71. 72. 73. 74. 75. 76. 77. 78. 79.
80. 81. 82. 83. 84. 85. 86. 87.
88. 89. 90. 91. 92.
171
B. 0. Lindgren and H. Mikawa, Acta Chem.Scand., 11:826-835 (1957). T. Higuchi, Y. Ito, and I. Kawamura, Phytochemistry, 6:875-881 (1967). H.A. Stafford, PlantPhysiol., 37643-649 (1962). Y. San0 and A. Sakakibara, Mokuzai Gakkaishi, 16:81-86 (1970). S. Omori and A. Sakakibara, MokuzaiGakkaishi, 20:388-395 (1974). H.Nimz, Chern. Ber., 98:3153-3159 (1965). A.Yamaguchi, MokuzaiGakkaishi, 19:185-193 (1973). A. Sakakibara, H. Takeyama, and N. Morohoshi, Holdorsch., 20:45-47 (1966). T. Higuchi, H. Nakatsubo, and Y. Ikeda, Holdorsch., 28: 189-192 (1974). E. Adler and S. Yllner, Acta Chem. Scand., 7:570 (1953). K. Lundquist and R. Lungren, Acta Chem. Scand., 26:2005-2023(1972). M. Aoyama and A. Sakakibara, Mokuzai Gakkaishi, 24:422-423 (1978). T. Popoff and 0. Theander, Phytochemistry, 142065-2066 (1975). J. Gierer and S. S6derberg. Acta Chem. Scand., 13:127-137 (1959). J. Marton, E. Adler, and K. I. Person, Acta Chem. Scand., 15:384-392 (1961). E. Adler and J. Marton, Acta Chem. Scand., 13:75-96 (1959). Y. Hachihama, K. Nira, and T. Kyogoku, Kogyo Kagaku Zasshi, 47209-215 (1944). H. Mikawa, K. Sato,C.Takasaki,and K. Ebisawa, Bull.Chem. Soc. Japan, 28:653-660 ( I 955). K. Freudenberg and K. Dall, Naturwiss., 22:606-607 (1955). K.V. Sarkanen and C. Schuerch, Anal. Chem., 2 7 1245-1250 (1955). K. Freudenberg,, in Fortschritte d. Chem. org. Naturstoffe, XI, Zechrneister, Springer-Verlag, Berlin-Heidelberg, pp. 43-82 (1954). E. Adler and S. Hernestam, Acta Chem. Scand., 19:319-334 (1955). A. Bjorkmanand B. Person, Svensk Papperstidn., 60:285-292 (1957). A. Okay, Hul~ursch.,24:172-175 (1970). D. R. Robert and G. Brunow, Holdorsch., 3835-90 (1984). H.-M. Change, E. B. Cowling, and W. Brown, Holdorsch., 29:153-159 (1975). P. Miinsson, Hol$orsch., 37143-146 (1983). D. S. Argyropoulos, J. WoodChem.Technol., 14:65-82 (1994). 0. Faix, C. Grunwiind, and 0. Beinhoff, Hol$orsch., 46:425-432 (1992). 0. Faix, D. S. Argyropoulos, R. Danielle, and N. Vincent, Holdorsch., 48:387-394 (1994). E. Adler and K. Lundquist, Acta Chem. Scand., 15:223-224 (1961). K. Freudenberg, C.-L. Chen, J. M. Harkin, H. Nimz, and H. Renner, Chem. Commun., 224 ( 1965). M. Aoyama and A. Sakakibara, Mokuzai Gakkaishi, 22591-592 (1976). E. Adler, S. Delin, and K. Lundquist, Acta Chem. Scand., 13:2149-2150 (1959). E. Adler and J. Gierer, Acta Chem. Scand., 9534-93 (1955). J. Gierer, Acta Chern. Scand., 8:1319-1331 (1954). J.Gierer, Chem.Ber., 80257-262 (1956). E. Adler, H.-D. Becker, T. Ishihara, and A. Stamvik, Holdorsch., 20:3-11 (1966). H.-D. Becker and E. Adler, Acta Chem. Scand., 15:218-219 (1961). T. Higuchi, M. Tanahashi, and F. Nakatsubo, Wood Res. (Kyoto), 54:9-18 (1972). K. Freudenberg, J. M. Harkin, and H. K. Werner, Chem. Ber, 97:909-920 (1964). E. Adler, G. E. Miksche, and B. Johanson, Holtforsch., 22:171-174 (1968). E. Adler, J. M. Pepper, and E. Eriksoo, Ind. Eng. Chem, 49: 1391-1392 (1957). S. Larsson and G. E. Miksche, Acta Chem. Scand., 25:647-662 (1971). M. Erickson, S. Larsson, and G. E. Miksche, Acta Chem. Scand., 27:903-914 (1973). H.Nimz, Chem. Ber, 98:3160-3164 (1965). K.Lundquist, G. E. Miksche, and I. Berndtson, Tetrahedron. Lett., 46:4587-4591 (1967). G. Aulin-Erdtman and L. Haghom, Svensk Papperstidn., 61:187-210 (1958). C.-L. Chen,InauguralDissertation,UniversitatHeidelberg,Heidelberg,Germany, pp. 1-75 ( 1962).
172 San0
93. 94. 95. 96. 97. 98. 99. 100. 101.
102. 103.
104. 105.
106. 107. 108.
and
Sakakibara
K. FreudenbergandC.-LChen, Chem. Ber., 100:3683-3688(1967). S. Larsson and G. E. Miksche, Acru Chem Scund., 25:673-679 (1971). H. Nimzand K. Das, Chem. Bes, 1042359-2380(1971). S. Yasuda and A. Sakakibara, MokuzaiGukknishi, 23:383-387 (1977). K. Freudenbergand D. Rasenak, Clzem. Res, 86:755-758 (1953). H. Nimz and H. Gaber, Chem. Bes. 98:538-539(1965). S. Omori and A. Sakakibara, MokuzaiGakkuishi, 17464-467 (1971). S. Omori and A. Sakakibara, Mokuzni Gakkaishi, 21:170-176 (1975). K. Ogiyama and T. Kondo, Mokuzai Gnkknishi. f4:416-420 ( 1968). K. Sudoand A. Sakakibara, MokuzaiGakknishi, 20:396-401(1974). S. Yasuda and A. Sakakibara, MokuzniGukkaishi, 22:606-612(1976). K. Freudenberg, Z. Angew. Chem., 52362-366(1939). B. Leopold, Acrn Chetn. Scnnd., 6:38-48 (1952). B. Leopold and J. L. Malmstrom, Actcl Chem. Scund., S:936-940 (1951). J. C.Pew, J . Am. Chern. Soc.. 77:2831-2833(1955). D. L. Brink, Y. T. Wu, H. P. Naveau, J. G. Bicho, and M. M. Merriman, nippi, 55:719-721
( 1972). 109. H. P. Naveau, Y. T. Wu, D. L.Brink, M.M. Merriman,and J. G. Bicho, 72ppi. SS:13561361 (1972). 110. S. Larsson and G. E. Miksche,Acta Chern. Scand., 2/:1970-1971 (1967). I 1 1. M. Eriksson, S. Larsson, and G. E. Miksche, Actu Chem. Scancl., 2 7 127-140 (1973). 112. S. Larsson and G. E. Miksche, Actu Chern. Scand., 233337-3351(1969). 113. S. Larsson and G. E. Miksche, Actu Chem. Scatzd., 26:20-31 (1972). 114. S. Yasuda and A. Sakakibara, Mokuzui Gakkuishi, 23: 114-117 (1977). 1 15. M. Matsukura and A. Sakakibara, Mokuzni Gakknishi, 19:17 1-176 (1973). 116. K. Sudo. B. H. Hwang, and A. Sakakibara, MokuzaiGakkaishi. 24424-425 (1978). 117. B. H. Hwang, A. Sakakibara, and M. Miki, Hol7forsch., 35:229-232 (1981). 118. K. Miki, V. Renganathan, and M. H. Gold, Uiochenzistt-y, 25:4790-4796 (1986). 119. K. Freudenberg, in Rrnnin, Cellulose, Lignin, Springer-Verlag,Berlin, p. 133 (1933). 120. E. E. Brauns and D. A. Brauns, in The Chemistry of Lignin, Academic Press, New York, p. 626 ( 1960). 121. B. H. Hwang and A. Sakakibara, Hol
Chemistry of Lignin
173
143. H. Nimz, U. Tschirner, and M. Roth, in 1983 Int. Symp. on Wood and Pulping Chernistv, Tsukuba, Japan, Vol. I , p. 90 ( I 983). 144. U. Westermark, B. Samuelsson, and K. Lundquist, Res. Chem. Intermed., 21:343-352 (1995). 145. K. M. J. Barrow, R. E. Ede,and I. D. Suckling, in 7th Int. Syntp. on Wood and Pulping Chemistry, Vol. I , pp. 73-81 (1993). 146. J . Sipil,G. Brunow, and P. Tunninen, in 7th Int. Symp. on Wood ctnd Pulping Chemistry, Vol. 3, p. 12 ( 1 993). 147. Y. Sano and A. Sakakibara, Mokuzai Gakkaishi, 31: 109-1 I8 (1984). 148. Y. Sano, Mokuzai Gakkaishi, 35:813-819(1989). 149. M.Bardet, D. Robert,and K. Lundquist, Svensk Papperstdn., 6:61 (1985). 150. L. Lin, M. Yoshioka, Y. Yao, and N. Shiraishi, in Abstr. 46th Annual Meeting of the Japan Wood Research Society, Kumamoto, Japan, p. 278 (1996). l 5 l. K. Lundquist and R. Lundtgren, Acta Chern. Scand., 26:2005-2023 (1972). 152. K. Lundquist, Acta Chern. Scand., 27:2597(1973). 153. E. Adler and K. Lundquist, Acta Chenz. Scand., 17:13-26 (1963). 154. K. Lundquist and G. E. Miksche. Tetrcthedron Lett., 2131 (1965). 155. H. Nimz, Chem. Ber., 102:799-810(1969). 156. C. Lapierre, B. Monties, and C. Rolando, J . Wood Chem.Technol., 5:277-292 (1985). 157. C. Lapierre and B. Monties, Holiforsch., 40:47-50(1986). 158. C. Lapierre, B.Pollet, and B. Monties, Holiforsch., 4 5 - 6 8 (1991). 159. N. Terashima,R. H. Atalla, S. A. Ralph, L. L.Landucci, C. Lapierre,and B. Monties, Holiforsch., 50:9- 14 (1 996). 160. A. Sakakibara, T. Sasaya, K. Miki, and H. Takahashi, Holzj-orsch., 41:1-11 (1987). 161. M. Erickson, S. Larsson, and G. E. Miksche, ActaChem. Scund., 27:903-914 (1973). 162. S. Larsson and G. E. Miksche, Acta Chern. Scand., 25:647-662 (1971). 163. K. Freudenberg, Holiforsch., 18:3-9(1964). 164. K. Freudenberg, Hokforsch., 18:166- 168 (1 964). 165. K. Freudenberg, Science, 148595-600(1965). 166. K. Freudenberg and A. C. Neish, in Molecular Biology, Biochemistry and Biophysics, Vol. 2, Springer-Verlag, Berlin-Heidelberg, p. 103 (1968). 167. E. Adler, Wood Sci. Technol., /1:169-218(1977). 168. W. Glasser, in Pulp and Paper, 3rd ed., Vol I (J. P. Casey, ed.), Wiley, New York, pp. 39I l l (1980). 169. A. Sakakibara, Wood Sci.Technol., 1489- 1 0 0 (1980). 170. H. Nimz, Angew. Chem., 13313-321(1974). 171. B. J. Fergus and D. A. 1. Goring, Post-Grad. Res. Rep. No. 12, McGill University, Montreal, Quebec, Canada (1968). 172. M. Matsukura and A. Sakakibara, Mokuzai Gakkaishi, 15:35-39 (1969). 173. K. V. Sarkanen, in Lignins (K. V. Sarkanenand C. H. Ludwid, eds.), Wiley-Interscience, New York, p. 154 ( 1 97 1 ). 174. W. A. Cote, B. W. Simon, and T. E. Timmell, Svensk Papperstidn., 69547-558 (1966). 175. K. P. Kringstad andC. W. Chang, Tappi, 52:2382-2385(1969). 176. F. Yaku, Y. Yamada, and T. Koshijima, Holiforsch., 30: 148-156 (1976). 177. 0. Eriksson and B. 0. Lindgren, Svensk Papperstidn., 80:59-63(1977). 178. R. Simonson, Svensk Papperstidn., 74:153-165(1971). 179. D. FengelandM. Przyklenk. Svensk Papperstidn., 78:617-620 (1975). 180. 0. Eriksson and D. A. I. Goring, Wood Sci.Technol., 14:267-279 (1980). 18I . K. Freudenberg and G. Grion, Chrrn. Ber., 92: 1355- 1363 (1959). 182. K. FreudenbergandJ. M. Harkin, Chem. Ber, 93:2814-1819(1960). 183. E. F. Brauns, J . Am.Chem. Soc., 61:2120-2127(1939). 184. K. Freudenberg, Angew. Chenz.,68:84-92(1956).
This Page Intentionally Left Blank
Chemistry of Cell Wall Polysaccharides Tadashi lshii and Kazumasa Shimizu Forestry and Forest Products Research Institute, Ibaraki, Japan
1.
INTRODUCTION
Cellulose and hemicellulose are major cell wall polysaccharides in woody plants which consist mainlyof lignified secondaryxylem.Theirchemicalstructureshavebeenwell characterized [ 1-41. Recent studies have revealed important biological and physiological functions of the primary cell wall polysaccharides in plant growth and regulation [5-71. Significant differences exist in polysaccharide composition of the primary cell walls and the lignified secondary walls. In this chapter, the structure and functions of cell wall polysaccharides, particularly pectin and hemicellulose, in growing tissue are discussed.
II. PRIMARY CELL WALL COMPONENTS The primary cell wall consists of two phases, a microfibrillar phase and a matrix phase. As shown in Table I , the primary cell walls consist of pectin, hemicellulose, cellulose, and a small amount of glycoproteins and phenolics. Polysaccharide compositions of primary cell walls are very similar in hardwoods(angiosperms)andsoftwoods(gymnosperms) (Table 2) [8], although the secondary wall polysaccharide compositions of these two divisions are different [4]. Traditionally, polysaccharides are classified as follows: pectins are polysaccharides extracted from cell walls by hot water, ammonium oxalate, weak acid, or chelating reagents; hemicelluloses are not extracted by weak acids but are by relatively strong alkali. The wall residue remaining after alkali extraction is mainly cellulose. This classification based on extraction procedure is convenient to use, but it is not always appropriate. For instance, pectic polysaccharides can be defined as galacturonic acid-containing polysaccharides [9]. Using this structural definition, pectic polysaccharides are extracted with both chelating reagents and with alkali. The a-cellulose fraction also contains residual galacturonic acid residues. The subdivision of matrix polysaccharides into pectin, hemicellulose, and cellulose is, however, useful (see Section IV).
175
lshii and Shimizu
176
TABLE 1
Primary Wall Components
Phase
Components
Microfibrillar Matrix"
Xylan
Cellulose (p-1,4-glucan) Pectins
Rhamnogalacturonan I Arabinan Galactan Arabinogalactan I Homogalacturonan Rhamnogalacturonan I1
Hemicelluloses Glucomannan Mannan Galactomannan Glucuronomannan Xyloglucan Callose (p-1.3-glucan) p- 1,3-, p- 1,4-glucan Arabinogalactan I1
ensin
Proteins
Phenolics
acid
Arabinogalactan protein Others, including enzymes Ferulic Others, e.g., coumaric acid, truxillic acid
"NB: Not all these matrix components are found in all cell walls. Source: Ref. 19.
111.
MONOSACCHARIDE RESIDUESCOMMONLY FOUND IN PLANT CELL WALLS
The most commonly occurring sugars found in cell wall polysaccharides are shown in Fig. 1. The carbonyl (aldehydo or keto) carbons of reducing sugars form acetal or ketal linkages, called glycosidic linkages. A glycosidically linked sugar is called a glycosyl residue; e.g., 4-linked glucosyl residues are glucosyl residues glycosidically linked at C- 1 and also have another glycosyl residue attached to them at C-4. In this chapter the following abbreviations are used: Glc = glucose; Gal = galactose; Man = mannose; Xyl = xylose; Api = apiose; Ara = arabinose; Rha = rhamnose; Fuc = fucose; GlcA = glucuronic acid; GalA = galacturonic acid; AceA = aceric acid; Kdo = 3-deoxy-~-manno-octulosonic acid; Dha = 3-deoxy-~-lyxo-2-heptulosanic acid; p = pyranose ring form; f = furanose ring form.
IV.
PURIFICATION OF PRIMARY CELL WALLS AND ISOLATION
OF POLYSACCHARIDES Xylem differentiating zones of woody plants, commonly called cambial tissues, contain primarywallsandmiddle lamella. Collection of cambial tissues for chemical analysis requires many young trees and much time-consuming work. The cambial tissues of aspen (Populus tretnuloides), basswood (Tilia umericarzn) [ 10- 141, and sugi (Cryptotneria jap o n i c a ) [ 151 were isolated and their cell wall polysaccharides were well characterized.
a 9
TABLE 2
Major Polysaccharides of Primary Cell Walls a
Dicots Suspension-cultured sycamore cell"
0'
z u)
Gymnosperms Aspen Cambial tissueh
Suspension-cultured Douglas-fir cells'
Sigi cambial tissue"
wt % of cell wall
Polymer
0
z ij: (P
u)
Cellulose Hemicellulose
Pectin
"From "From 'From "From
Ref. Ref. Ref. Ref.
5. 10.
8. 15.
Xyoglucan Xylan Glucomannan Homogalacturonan Rhamnogalacturonan-I Rhamnogalacturonan-I1
30 25 5 15 15 5
22 6 11 1
147
23 15 2
j2Z
35 18 5 8
178
lshii and Shimizu
bH OH p-D-Glucopyranose
bH
OH a-L-Rhamnopyranose
a-L-Fucopyranose
p-D-Xylopyranose
p-D-Mannopyranose
OH a-L-Arablnofuranose
CYOH
COOH
COOH
OH
I
OH p-D-Galactopyranose
64 CHpOH
OHOH
p-D-Aplofuranose
I
I
OH a-D-Galactopyranosyluronicactd
'0
OH p-D-Glucopyranosyl-uro nic acid
CH2OH
I
COOH
HO-C
H
OH 2-keto3-deoxy-D-manno2-octulosonic acld (Kdo)
"
O
H COOH
3-dWxY-D-l~~o-2-hep tulosaric acid (Dha)
OH p-L-Aceric acld
FIGURE 1 Structure of monosaccharides commonly found in the cell wall.
Suspension-cultured cells are also a good source for preparing primary cell walls. Albersheim and his co-workers [ 161 have used suspension-cultured sycamore (Acer pseudoplaranus) cells for studying the structures and functions of primary cell walls. Suspensioncultured cells of woody plants can be easily obtained from young leaves, seedlings, and cambial tissues. Procedures for preparation of cell walls from suspension-cultured cells (Fig. 2 ) and isolation and fractionation of polysaccharides are described byYork et al. [ 161, while alternative procedures for preparing cell wall materials from fresh tissues have
Chemistry of Cell Wall Polysaccharides
h
3
aJ
.e
5 c Ir
M
0
0
2 v)
v
8
B
3 M
aJ
v)
Y
:a 2&
179
lshii and Shimizu
180
been proposed by Selvendran and O’Neill [ 171 (Fig. 3). The sequential extraction of pectin and hemicellulose from cell wall material is shown in Figs. 4 and 5, respectively. These approaches gave an enormous amount of information on the structure of individual polysaccharides, but they also have their limitations. One notable disadvantage is that certain bonds in the wall are destroyed in order to extract its components [ 18,191, which may make it difficult to observe important covalent bonds of the polysaccharides. This drawback might be partly overcome by comparing different extraction methods and especially by comparing chemical and enzymatic extraction methods. A second limitation is that cell wallpolysaccharidesareoftenheterogeneouswithrespectto their primary structure and molecular size. Extraction and purification of polysaccharides may result in only partial recovery of a particular type of molecule, and the recovered material may not be representative of the whole. This ultimately leads to a distorted picture of the overall structure of the component. Despite the many limitations of studying cell wall polysaccharides, extremely powerful tools for analyzing small amounts of complex carbohydrates are currently available. Theseinclude capillary gas-liquidchromatography-massspectrometry (capillary GCMS), liquid chromatography-mass spectrometry (LC-MS), fast-atom-bombardment mass
Fresh tissue Homogenize in 1.5%(w/v) SDS (2.5 fresh weight) containing 5 mM Na,S20s at 5-10°C until homogeous Filter and wash (x 2 ) in 0.5% (w/v) SDS containing 3 mM dm-3Na2SzOS
t
Supernatant: containing cell contents and watersoluble cell wall components
Residue
+
Ball mill at 1°C in 0.5%(w/v) SDS containing 3 mM dm-3Na,S,05 Centrifuge andwash in water (x 2 )
1
+
Supernatant:containing water-soluble pectic substances
Residue
(1) Extract with 90%(v/v) DMSO to remove starch (2) Wash in distilled water, and dialyse
Purified cell wall material (Yield, 0.5-2%(w/w) of fresh material)
FIGURE 3 Procedure f o r (he preparation of cell wall material from fresh tissue. (From R d . 17.)
181
Chemistry of Cell Wall Polysaccharides
Cell wall material (1 g) CDTA-(1) Stir with 100 mLCDTA 50 mM, pH 6.5 for 5 h at 20°C Centrifuge and wash lx with distilledH 2 0 Add washingsto supernatant (SIN) Residue
SIN
filter through glassfiber paper, dialyse, concentrate under reduced pressurebelow 40"C, dialyse and concentrate CDTA-( 1) soluble
I
CDTA42) Re-extract withCDTA as above for 2 h Centrifuge and wash as above
t Residue
SIN
Filter, dialyseand concentrate CDTA-(2) soluble Na2C03-(1) Stir with 100 mL 50 mM Na2C03+ 2 0 mM NaBH, (0,-free unde Ar) for 2 0 h at 1'C Centrifuge and wash withHzO
t
Residue
UN
Na2C03-(2) Re-extract with 50 mM Na2C03 as above for 2 h at 20°C Centrifuge and wash
Extractwithalkali(Fig.
FIGURE 4
5)
Extraction of pectic polysaccharides
1
Filter, adjustpH to 5 with acetic acid, dialyse and concentrate Na2C03-(l)-(cold)-soluble
SIN Filter,etc.,asabove Na2C03-(2)-(room temperature)-soluble from cell wall material. (From Ref. 17.)
lshii and Shimizu
182
Depectinated CWM
Stir with 75-100 mL 02-free 0.5M KOH + 10 mMNaBH, under Ar for 2 h at 20°C Filter under suction
v
Residue
Filtrate, adjust pH to 5 with acetic acid, dialyse and concentrate 0.5 M KOH-soluble Stir with 75-100 mL 02-free 1 M KOH + 10 mMNaBH, under Ar for 2 h at 20°C Filter under suction
v Residue
Filtrate, adjust pH to 5 with acetic acid, dialyse and concentrate 1 M KOH-soluble
Extract with 75-100 mL 0,-free 4 M KOH + 10 mMNaBH, under Ar for 2 h at 20'C
l+
Filter under suction
t
Residue a-Cellulose
Filtrate, treat as above
4 M KOH-soluble
FIGURE 5
Extraction of hemicellulose from depectinated cell wall material.
(From Ref. 17.)
spectrometry (FAB-MS), electrospray ionization mass spectrometry (ESI-MS), matrix-associated laser-desorption time-of-flight mass spectrometry (MALDI-TOF-MS), and highresolution nuclear magnetic resonance (NMR) spectroscopy. Purified enzymes for selectively hydrolyzingglycosyllinkages are also available. These tools provide much information regarding the structure and function of cell wall polysaccharides, even though there are always problems associated with isolating complex polysaccharides and elucidating their exact structural features.
Polysaccharides Chemistry Wall of Cell
183
Several methods are available for the analysis of intact cell walls. Solid-state NMR and Raman spectroscopy give useful information. Immunocytochemical study using goldlabeled antibodies and wall-degrading enzyme also yields information about the distribution of cell wall components.
V.
STRUCTURAL ANALYSIS OF POLYSACCHARIDES
Polysaccharides are characterized by glycosyl composition and glycosyl-linkage analyses. Figure 6 is a flow chart for the sequencing of the neutral and acidic polysaccharides.
A.
MonosaccharideComposition
1. Acid Hydrolysis Plant cell wall polysaccharides contain at least 12 monosaccharides which are linked by a variety of glycosyl linkages. Theirsusceptibility to acid hydrolysis varies [20]. Therefore, a single hydrolysisprocedurecannotprovidequantitativehydrolysis of everyglycosyl linkage. Furthermore, the monosaccharides released by acid have different acid stabilities. Neutral noncellulosic polysaccharides can be hydrolyzed quantitatively using 1 M H,SO, for 2.5 h at 100°C, or 2 M trifluoroacetic acid (TFA) for 2 h at 120°C [21]. The cellulose Polysaccharide Glycosyl composition Analysis Glycosyl linkage analysis
NeutraVAcidic
I
I
I
Partially degrade
Carboxyl-reduce
I
Methylate
I
I
(chemiclally, enzymatically) Oligosaccharides
Gel permeation Ion-exchange HPLC Purified oligosaccharides
'"C-NMR
FIGURE 6
NeutraiIAcidic
Methylate I
Carboxyl-reduce I
I
Partially degrade Reduce Realkylate
Alkylatedoligoglycosyl
alditol
l
I
Reversed-phase HPLC
Hnarysls
Flow chart lor sequencing polysaccharides. (From Ref. 17.)
184
lshii and Shimizu
is first degraded with 72% H,SO, for 2 h at 20°C and then hydrolyzed completely by 1 M acid for 4 h at 100°C [ 171. TFA is more convenient than H,SO, because it is volatile and gives higher recovery of neutral and acidic sugar residues than H,SO,. Ketoses are very acid-labile sugars and degrade during hydrolysis of polysaccharides. Kdo and Dha can be released by 1 M acetic acid at 40°C for 16 h and 2 M TFA at 120°C for 5 min, respectively [9]. Kdo and Dha are specific components of rhamnogalacturonan-I1 (RG-II), which are present in all higher plants [9].
2. AlditolAcetatesMethod Neutral sugars released by acid hydrolysis are reduced with sodium borohydride (NaBH,), acetylated, and analyzed as alditol acetates by gas-liquid chromatography (GLC) [ 161. The alditol acetates are well separated from each other by GLC and determined quantitatively (Fig. 7).
3. TrimethylsilylEthers of MethylGlycosides Polysaccharides that contain acidic sugarresidues are subjected to methanolysisand methyl glycosides of neutral sugars and also methyl ester of uronic acid residues, which are converted into trimethylsilyl (TMS) derivatives. TMS derivatives can be analyzed by GLC with capillary column [l61 (Fig. 8).
B. Glycosyl-LinkageAnalysis Methylation analysis gives information about the glycosyl linkages of the polysaccharides. The procedure includes permethylation of all free hydroxyl groups, hydrolysis, reduction of partially methylated monosaccharides, and acetylation. The Hakomori method, using sodium dimethylsulfinyl anion (dimsyl anion) in dimethylsulfoxide, is commonly used for permethylation [22]. Potassium dimsyl anion is more easily prepared [23]. Blakeney and Stone [24] prepared the lithium carbanion from butyllithium, which is available in a much purer form than the alkali metal hydrides, thus providing a clearer chromatogram. Ciucanu and Kerek [25] reported a new methylation method in which powdered sodium hydroxide and iodomethane are added to carbohydrate in dimethylsulfoxide. Methylation with sodium hydroxide and iodomethane in SOz-diethylamino-dimethylsulfoxide is useful for cellulose and lignified samples [26]. Acidic polysaccharides have to be reduced either before or after methylation to analyze their uronic acids as partially methylated alditol acetates (PMAAs). The uronic acids are reduced with a deuterated reagent so that they can be distinguished by mass spectrometry. Water-soluble polysaccharides whose carboxyl acids have been activated with carbodiimide can be reduced with sodium borohydride and subjected to methylation analysis. Alternatively, the methylated polysaccharides are readily reduced by refluxing with lithium aluminumdeutride in dichloromethaneether [17]. York et al. reported that lithium triethylborodeutride in tetrahydrofuran is highly effective onmethyl esterified methylated polysaccharides [ 161. Methylated polysaccharides are hydrolyzed with 2 M TFA for I h at 120"C, reducedwithsodiumborodeutride,andacetylated.PMAAs are separatedon capillary GLC columns. PMAAs can be easily identified from the pattern of fragment ions produced by electron-impactmassspectrometry[27].ThePMAAsderivedfrom arabinoxylan are shown in Fig. 9.
185
Chemistry of Cell Wall Polysaccharides
l 4
x
X
I
I
I
I
I
1
I
Time (min) FIGURE 7
GLC of alditol acetates of neutral sugars.
VI.
MATRIX POLYSACCHARIDES
A.
Pectic Polysaccharides
The primary cell walls of dicots have a relatively high content (-35%) of pectic polysaccharides. The primary wall and middle lamella are rich in pectic polysaccharides. The most characteristic glycosyl residue of pectic polysaccharides is galacturonosyl residue. Rhamnosyl, arabinosyl. and galactosyl residues are also present. The rhamnosyl residues are closely associated with galacturonosyl residues in integral components of the polysaccharides. Arabinosyl and galactosyl residuesarecomponents of arabinan and galactan, which are covalently attached as side chains to a rhamnogalacturonan backbone 191. Pectin is covalently linked to phenols 1281, and may also be linked to protein 128,291 and lignin [301. Three pectic polysaccharides have been isolated and characterized. These are homogalacturonan,rhamnogalacturonan I (RC-I), and rhamnogalacturonan I1 (RG-11). Hornogalacturonan, oligogalacturonides [degree of polymerization (DP), between I and 31, R C I, and RG-I1 were solubilized from suspension-culturedsycamore cell walls with CY-l,
lshii and Shimizu
186
0
f
FIGURE 8
C
E
GLC of TMS derivatives of neutral and acidic sugars.
(From Ref. 16.)
4-endo-polygalacturonase (EPC) treatment. These results suggest that homogalacturonan is covalently attached to RG-I and RG-I1 in vivo [9].
1. Homogalacturonan Homogalacturonan is a homopolymer of a- 1,4-linked galacturonic acid (Fig. 10). Oligogalacturonides having DP 2- 12 were prepared from cell walls of soybean by partial acid hydrolysis and isolated by ion-exchange chromatography [3l]. Recently, oligogalacturonides (DP 5-20) were separated by high-performance ion-exchange chromatography on a Carbo Pac PA1 column (Dionex) (Fig. 11). The carboxyl groupsof many of the galacturonosyl residues of pectic polysaccharides in cell walls are partly esterified [32], but the distribution of the methyl esters is unknown. Calacturonosyl residues are partially acetylated at 0-3 position [33]. Homogalacturonanshave structural roles in the plant cell walls, and oligogalacturonidesderivedfromthehomogalacturonanhave biological activities [34],including elicitation of defense responses, influence on plant growth and development, and promotion of rapid changes in ion flux (Table 3). 2. Rhamnogalacturonan I (RG-I) RG-I was solubilized from suspension-cultured sycamore cell walls after treatment with EPG[9].Glycosylcomposition analysis of RC-Ishowed that arabinose,galactose,galacturonic acid, and rhamnose are its major monosaccharide constituents (Table 4). Small amounts of fucoseare present. Glycosyl-linkageanalysis,followingreduction of the methyl esterified galacturonic acid residue, established that RC-I is a complex, branched
187
Chemistry of Cell Wall Polysaccharides
a
$
"
o
~
o
9
OH
OH
o \
~
G J + Me0
OH
OH
J
o
Q
Methylation
g
o
\
COOMe
MeO
M
OMe
OMe Reductbn of uronate AcM hydrolysls
CHDOAc
CHDOAc
M&$"" AcO
AIS{-::
CH20Me CH20Ac 1-Araf
t
Reduction Acetylation
CHDOAC
M e 0 i o M e OAC
OAc CH20Ac
CH20AC 3,4-Xylp
CHDOAc
+XYlP
FIGURE 9 Partiallymethylatedalditolacetates
24-XYlP
from arabinoxylan.
188
lshii and Shimizu
-+4)-a-~GalpA-(l+4)-a-~GalpA-(l-+4)-a-~-GalpA-(l+4)-a-~-GalpA-(l+4)-a-~GalpA-(l-+ FIGURE 10 Structure of homogalacturonan. Galacturonic acid residues are partly esterified.
pectic polysaccharide (Table 5 ) composed of the repeating disaccharide +4)-cu-D-GalpA(1+2)-cw-~-Rhap-(1+ (Fig. 12-1). Typically, 50% of the 2-linked rhamnosyl residues are submitted at 0-4, but the pattern of side-chain substituents along the backbone is not clear. Calacturonosyl residues of RC-I are acetylated on 0 - 2 and 0 - 3 135-371. Acetylated RCI oligomers were obtained from the walls of bamboo shoot by Driselase hydrolysis (37). RC-I has a DP of about 2000, even after extraction from the walls by EPG treatment 191. RC-I has a number of different side chains, attachedto the 0 - 4 position of rhamnosyl residues. Lithium degradation of the galacturonosyl residues in RC-I released oligoglycosy1 side chains attached to 0 - 4 of 2-linked rhamnosyl residues (Fig. 12-2) 191. The cell walls of suspension-cultured Douglas fir (Pseudorsugu menziesii) cells [8] and the cambial tissue of sugi 1381 have a RG-I with a structure very similar to sycamore RC-I. Pectic polysaccharides extracted from various tissues and plants contain RC-I with a variety of side chains. Their structures are remarkably conserved. It may be that cells produce RCI with different side chains depending on ages and difference in tissues. The RC-I may have some physiological functions in cells, but there is little evidence for this notion. Some walls [Chenopodiaceae, e.g., spinach (Spinncia oleraceu and sugar beet (Betu ~xdgaris)] contain esterified phenolics. Several feruloyl oligosaccharides wereisolated from enzymatic hydrolyzates of spinach suspension-cultured cell walls 139,401, spinach leaves [41], and sugar beet pulp [40]. They were identified to be 0-(2-O-trtrn.s-feruloyl-a-~-Ar~fl(1-+5)-~-Acaf (Fig. 13-1), 0-(6-O-rrc~ns-feruloyl-~-~-Galp)-( 1+ 4 ) - ~ - C a l p (Fig. 13-2, 0a-~-Araf-(1+3) 0-(2-O-rlun.s-feruloyl-~-~-Ar~f)-( l + 5 ) - ~ - A r ~ f(Fig. 13-3), and 5 - 0 rrc/n.s-feruloyl-c~-~-Araf-( 1 +3)-O-p-u-Xylp-( 1+4)-~-Xylp (Fig. 13-4). These feruloyl res-
540-
480420 -
- 360al
U7
6
3006
0
f
240-
I
U
1800
12060 -
0-
B
l
11
Polysaccharides Chemistry Wall of Cell TABLE 3 Biological Activities of
189 a-l ,4-Oligogalacturonides
Activity
dp“
Molar conc.h
Plant
Plant defense responses Induction of
phytoalexins
Induction of proteinase Inhibitors ligninInduction of
of
8-13 (12)’ 9-13 (13) ND* 2-20 20 8-11 (11) ND
-
-
5 1 0 - 4 10-5
10”
ofInduction P-1,3-glucanase ND Induction ND chitinase Induction of isoperoxidases ND Inhibition of hypersensitive response ND Elicitation NDof necrosis
Soybean Castor bean Parsley Tomato Tomato Cucumber Castor bean Parsley Tobacco Castor bean Tobacco Cowpea
Development and growth Inhibition of auxin-induced elongation Regulation of TCL morphogenesis: flower formation Induction of ethylene
Pea stem
>8 10-14 (12-14)
10”
>8 22
-
Enhancement of cell expansion and 100 separation Rapid responses at the plasma membrane and cell surface Efflux of K’ and influx of Ca’+ Rapid depolarization of plasma membrane and ND Induction of HzO,oxidative burst Enhancement of in-vitro phosphorylation of 34-kDa protein
Tobacco Tomato Pear Soybean
Tobacco Tobacco
12-15 1-7 and 10-20
Soybean 14-20
-I 0~-7
Tomato
‘Dp (degree of polymerization) range of oligogalacturonldes that show the designated biological activity. hOrder-of-magnitude estimatton of the concentratton of oligogalacturonldes that give the half-maximum biological response. The concentration is included only where purified oligogalacturonides are assayed. ‘Numbers in parentheses represent dp of most active oligogalactouronide. dND = dp of active oligogalacturonides not determined. Source: Ref. 34.
iduesareattached to arabinanandgalactan that are sidechains of RC-I in pectic polysaccharides.They may beinvolved in the cross-linking of pectin in cell wall (see Section VI).
3. Rhamnogalacturonan I1 (RG-11) RC-I1 is a polysaccharide composed of a 1,4-linked a-D-galacturonic acid backbone with both keto-sugars (i.e., ketoses) and aldehyde sugars (i.e., aldoses) in its oligosaccharide
lshii and Shimizu
190
Glycosyl Residue Composition of RG-I from the Walls of Suspension-Cultured Sycamore, and Douglas Fir
TABLE 4
Glycosyl Douglas Sycamore‘ Sycamoreb residue‘‘
fir”
Rha
16
9
9
Fuc
2
1 35 2 43 0 10
4 30
Ara XY 1
Gal Glc GalA
4
32 0 31 0
21
6 26
“Values expressed as mol%. hEndo-polygalacturonase-solubilizedRC-I. ‘NazCO,-solubilized RG-I. “LiCl-solubilized RC-l. Source: Ref. 9.
side chains. RG-I1 was for the first time isolated from the walls of suspension-cultured sycamore cells with EPG hydrolysis followedby size-exclusion chromatography [23]. The polysaccharide is composed of about 11 glycosyl residues and has extremely complicated glycosyl-linkage compositions (Tables 6 and 7) [9]. Aceric acid (3-C-carboxyl-S-deoxy-~xylose) (Fig. 1 ) was identified for the first time in nature as a component of RG-I1 [42]. Kdo and Dha (Fig. l), which are acid-labile molecules, were also identified as integral components of RG-I1 [9]. Partial acid hydrolysis of the RG-I1 gave several oligosaccharides (Fig. 14) [9,43]. Organization in RG-I1 of the oligosaccharides was elucidated by sophisticated sugar linkage analyses. Partial acid hydrolysis of methylated, carboxyl-reduced. and remethylated RG-11, in combination with selective deuteriomethyl labeling of those hydroxyl groups exposed by the partial acid hydrolyses, showed the points of attachment of oligosaccharides to the a-1A-linked galacturonosyl residues [9,44] (Fig. 15). The exact galacturonosyl residues in the homogalacturonan (Fig. 14-1) to which oligosaccharides 1, 2, 3, and 4 (Fig.14-2-5) are attachedhave not beendetermined. RG-I1is present in Douglas fir [S], sugi [38], rice (Oyvzra sativa) [4S], onion (Allium cepa] [46], kiwi fruit (Actinidin deliciosa) [47], bamboo shoot [48], and all other higher plants that have been examined [S]. Very recently a borate-RG-I1 complex was isolated from radish (Rq3hanu.s sativus) roots 1491, sugar beet pulp [SO], sycamore [SI], red wine [ S I ] , and bamboo shoot 1521. Boron (B) is knownto be an essential micronutrient for all higher plants [ S ] . Borondeficiencysymptoms first appear at growingpointsand are characterized by cell wall abnormalities (541. The finding that B selectively binds RG-I1 in pectin to form a crosslink (Fig. 16) implies that B-RG-I1 complex plays an essential role in cell wall architecture and cell formation. A pectic polysaccharide containing galacturonosyl and xylosyl residues (xylogalacturonan) (Fig. 17) was isolated from mountain pine pollen 1.551 and modified hairy regions of apple [ 5 6 ] . Xylogalacturonan was solubilized when the hairy region of polysaccharides was treated with rhamnogalacturonan hydrolase, which cleaves the backbone of RG-I but does not cleave xylogalacturonan. This result suggests that xylogalacturonan and RG-I is connected covalently in the wall.
Polysaccharides Chemistry Wall of Cell
191
Glycosyl-Linkage Composition of RC-I Isolated from the Cell Walls of Sycamore, Douglas Fir, and Maize
TABLE 5
48%
Glycosyl linkage" Rha
Fuc Ara
Sycamore Percent branched rhamnosyl residues fir
T
0
2 4 2,3 2,4 239
7.8
T
0.6 1.4
0.6
3,4
0
0
T
9.5 2.2 2.2 11.2
2.2
2 3 5
23 3s XYI Gal
1 .O
T
3.5 2.0
4 2.4
0 0
T
2 3 4 6 2,4 2.6 3.4 3,6 4.6 GlcA GalA
0 0 8.O
3.0 15.2 2.8 1.6 8.O
T T
4 2,4 3,4
6.3 0.6 2.7 8.4 7.5 6.3 1.2 0 l .2 2.4
1.1
0
0.9 3.4 l .4 1.1
0.7 0
0.5
1.3 0.6 0 10.6 2.0 2.4 0 2.8 0.4 2.6 8.0 3.2 5.9 0.3 0
0
0
8.1
6.6 2.9 3.9 11.3 8.1 6.6 2.5 1.4 6.5 0.8
1.o
2.2 2.9 4.4 0
0.2 0.4 0.6 1.5
0
0
0
1.6 15.2
4.4 30.6 0.2
0.6 12.5 0.2 1.9
1.o 0
1.1
Maize
0 1.1 0 t
0.4
2.8
11.8 2.1
0.5
t 0.5
13.4 t
17.2 19.8 6.8 7.4 t t t 15. I
0.8 4.2 4.9
1.o
15.1 0
5.7 0 0
0 0
14.9 0.8 2.5 13.0 l .4 6.1 1.1 1 .O 1.1
14.2 0.2 3.5 4.8 4.8 14.2 1.9
1.2
0.7
1.1 1.1
2.6 0
1.6
0 0' 0 0 0
0' 0 0 0
"Values expressed as mol%. Source: Ref. 9.
4.
Arabinans
Arabinans have been isolated from the tissues and cell walls of many plants [7]. It still remains unknown whether arabinans exist in growing tissue as separate homopolymer, or as covalently linked side chains of RG-I. Arabinans are highly branched molecules composed of a-lS-linked arabinofuranosyl residues that are more frequently substituted at 03 than at 0-2 (Fig. 18). Sycamore RG-I contains arabinosyl oligosaccharides (DP 2-20) attached to 0-4 of the 2-linked rhamnosyl residues in the backbone [36,58].
192
lshii and Shimizu
(1) +4)-a-~-GalpA(1-.2)-a-L-Rhap-(l--4)-a-D-GalpA(l-r2)-a-L-Rhap(l-
a-L-Fucp-( 1-2)-p-D-Galp( 1-r4)-p-D-Galp(l-r4)-Rhamnitol
a-L-Araf-(1+5)-a-L-Araf-( 1-+2)-a-L-Araf-(l-r3)-p-~-GaIp(1-.4)-Rhamnitol
Araf-[Araq,,-Rhamnitol
Galp-[Galp],,-Rhamnitol
FIGURE 12 Structure of rhamnogalacturonan-l: ( 1 ) backbone structure and (2) several side chains.
5. Galactans Some primary cell walls contain p-IP-linked galactans (Fig. 19) [7]. Galactose-containing oligosaccharidesattached to 0 - 4 of 2,4-linkedrhamnosylresidueswere isolated from sycamore RG-I [59,60] and tobacco RG-I [61].
Arabinogalactan Two types of arabinogalactan were isolated from plants (Fig. 20) [7]. Arabinogalactan I is a polysaccharide composed of a p- 1,4-linked galactosyl backbone that is substituted at 0-3 with short a-i,S-linked arabinosyl side chains. Arabinogalactan I1 is found in gymnosperms, especially in larches 1621. It is a highly branched polysaccharide containing p3, p-6-, and P-3,6-linked galactose with various amounts of arabinosyl, galactouronosyl, andglucuronosyl residues. Suspension-cultured plant cellshavebeenfound to secrete arabinogalactan protein into the culture medium 191. The polysaccharide portion is very similar to arabinogalactan 11. This polysaccharide may be covalently attached to hydroxyproline-rich proteins [62,63]. 6.
B. Xyloglucan Xyloglucan is the principal hemicellulose of the primary cell walls of dicotyledonous plants. It was first isolated and characterized from tamarind (7hmarindu.s indicu) seeds. The polysaccharidesformabluecomplexwith iodine. Thestructureandfunction of primary cell wall xyloglucan have been reviewed extensively [7,64,65]. The basic structure of this cell wall polysaccharide consists of a backbone of p-1,4-linkedD-ghCOSYl residues, with D-xylosyl side chains a-linked to 0 - 6 of some of the glucosyl residues. Some of the xylosyl side chains are extended by the addition of D - G a l j , ~ - F u c + 2 - a - ~ - G a l + to 0-
193
Chemistry of Cell Wall Polysaccharides
H.OH
' * O H OCH3
c=cH
b Lo (4)
FIGURE 13 Feruloyl oligosaccharides isolated from spinach and sugar beet cell walls.
194
lshii and Shimizu
TABLE 6 Glycosyl-Residue Composition of RC-I1 Isolated from
Different Plant Sources
RiceSycamore residue" Glycosyl 3.7 4.1
14.5 29.3
Rha Fuc 4.9 2MeFuc 5.3 Ara 2MeXyl 7.3 Apiose 9.0 Gal 12.3 GlcA GalA 26.7 Aceric acid Kdo Dha
2.8 3.5 10.0 4.8 12.2 9.0 3.2 31.2 3.5 3.5 3.5
15.3 4.1
10.0
10.2
6.3
6.7
+ + +
+ + +
"Values expressed as mol%. Source: Ref. 9.
TABLE 7
Glycosyl-Linkage Composition of RC-I1 from Different Plant
Sources" ~
~
~
ycamore linkagebGlycosyl Rha
T'
2 5.9 3 3.72 3
3.1 Fuc 5.52MeFuc Apiose Ara
5.3 9.0 5.8
GlcA
Tf
TP 2, T
2MeXyl Gal 5.6 GalA
T
3'
T
10.0
2,4 3,4 10.2 T 4 3.13,4 2.82,4 2,3,4
8.6
6.6 t
5 .O t
5.7 4.5 4.8 10.9 6.1 0 5 .O
4.5 5.24.9 6.5 0
10.3 6.08.8 7.3 4.6 1 .S
6.3
0
4.2 7.3 6.8 5.5 0
1.7 6.3
10.2 6.3 4.9 0 4.1 2.8
7.9 7.6 4.2
2.7 6.3
1.5
6.7
"5-LinkedKdo and 5-linked Dha are also present in these preparations and account for -5% of the material. hValues expressed as mol%. Source: Ref. 9.
Chemistry of Cell Wall Polysaccharides
195
a-D-GalpA-(l~4)-(a-D-GalpA]5.,-(1-4)-~-GalpA (1)
a-D-Galp 1
1
&
4
3 ~-D-GalpA-(l+4)-a-~-Fu~p(l+4)-p-~-Rhap(l+d)-Apif 3 2 2
t
t
1 2Me a-D-Xylp
a-D-GalpA
1
(2)
2Me a-L-Fucp 1
t 2 a-D-Galp(l-+2)-p-~-Acef-(l+3)-p-~-Rhap(l+3')-Apif
4
t 1 a-L-Arap 2
t 1
a-L-Rhap
(3) a-L-Rhap(l+5)-D-KDOp (4)
p-L-Araf-(l-.5)-D-DHAp (5)
FIGURE 14 Oligosaccharides releasedfromrhamnogalacturonan I1 bypartialacid
hydrolysis.
2. Structure of xyloglucan oligosaccharides and their nomenclature are shown in Fig. 21 [66]. In some tissues, the xyloglucan has been proposed to be composed of a repeating nonasaccharide unit (XLLG, Fig. 22-l), or of alternating nonasaccharide and heptasaccharide units (XXXG,Fig. 22-2) [7].Xyloglucan isolated from sycamore extracellular polysaccharides has acetyl groups [67,68], attached to the 2-linked P-galactosyl residues of thenonasaccharidesubunit. These P-galactosylresiduesweremono-0-acetylated and di-0-acetylatedat 0-6, 0-4, and 0 - 3 at degrees of 55-60%, 15-20%, and 2025%, respectively. Sycamore xyloglucan also contains arabinose residues. An arabinosecontainingheptadecasaccharidewas isolated fromsycamoreextracellularxyloglucan (XXFGAXXG, Fig. 22) [68]. The heptadecasaccharide was a combination of nona- and heptasaccharide components. An arabinosyl residue was glycosidically linked at 0-2 at
9
c
Q
196
i
4:-
.-.
v
4 P t
d
'c
h t
- 2n h + ci
h
n
'c
-2
U
dai
P b Q
lshii and Shimizu
8
i
0
cc
-L-Araf
1 97
Chemistry of Cell Wall Polysaccharides
+4)-a-~GalpA-(l+4)-a-~GalpA-(l-t4)-a-DGalpA-(l+4)-a-~GalpA-(l+4)-a-~GalpA-(l+
3
3
t
t
1
1
P-DXYlP
FIGURE 17 Structure of xylogalacturonan.
~5)-a-~-AraF(l+5)-a-~-AraF(1-15)-a-L-Araf(1+5)-a-~-AraF(l-15)-a-~-AraF(1+5)-a-~-Araf-(l~
3
3
2
t
1‘
t
1 a-L-Araf
1
1
FIGURE 18 Structure of arabinan.
+4)-p”alp-(1~4)-p-D-Galp-(l-t4)-p-PGalp-(l~4)-p-D-Galp(l+4)-(3-D-Galp-(1-14)-~-D-Galp-~l+ 3 3
t 1 a-L-Araf-(l+5)-a-L-Araf-(l+5)-a-L-Araf
FIGURE 19 Structure of galactan.
t 1 a-L-Araf
L-Araf
lshii and Shimizu
198
Arabinogalactan I
~3)-~-r>Galp(l~3)-~r>Galp(l-13)-~-r>Galp(l~3)-~-r>Galp~l~3~-~-r>Galp~l-13~-(3-~Galp(l~3)-
6
6
6
t
t
t
1 S-c-Galp
1 a-~-Araf-(l-13)-B-r>Galp
1 a-L-Araf-(l-13)-(3-r>.Galp
6
6
6
t
7
7
1
1
1 a-L-AraC(1-13)-(3-r>Galp
a-L-Araf a-~-AraF(1+3)-p-r>Galp
6
6
t
7
1 a-L-AraF(1+3)-p-r>.Galp 6
1
t 1 a-L-Araf Arabinogalactan II
FIGURE 20
Structures ofarabinogalactan I and arabinogalactan 11.
the nonreducing-endglucosylresidue of the heptasaccharidecomponent of theheptadecasaccharide. Xyloglucan oligosaccharides containing from 17 to 20 glycosyl residues were isolated andcharacterized[69-7 l]. Extensive structural characterization of xyloglucan oligosaccharides from various cell walls led to a ‘H-NMR database that allows the complex signals of xyloglucanderivedfromvarious plant species to be assignedwith relative ease [72,73]. The xyloglucans in Solanaceae species have unusual structures. For example,xyloglucansfrom Nicotiniatabacum and Solanumtuberosum do notcontain fucose, but have arabinose instead [64,74]. Xyloglucans in monocot cell walls have fewer substituted xyloseresiduesthan in dicotxyloglucans. Some monocotxyloglucanshave galactosyl-containing side chains like dicot xyloglucans. The presence of fucosyl-containing side chains has not been clearly established in monocot xyloglucans [64]. Monocot xyloglucan contains ester-linked ferulic acid residues [75]. A feruloyl xyloglucan disaccharidewas isolated frombambooshoot cell walls[76](Fig.23).This indicates that xyloglucan may have diferuloyl groups that cross-link xyloglucan-polysaccharides networks in the wall. Xyloglucan has a structural role in plant cell walls. Some or most of the cell wall xyloglucan is hydrogen bonded to cellulose (Fig. 24), as strongalkali is required to extract xyloglucan from cell walls and from pure cellulose in vitro [64]. Xyloglucan binds rapidly and strongly to cellulose in vitro. The binding of xyloglucan to cellulose fibers in the cell
3 (P
Abbreviations Structure Glc+Glc-tGlc-tGlc
t
Xyl
Old
New
XG10
XLFG
xt I xt I
t XG9
XXFG
x
x71 Gal
Fuc
Fuc
FG
XG9n
XLLG
t
t
Xyl
Gal Gal
t
Xyl
t
t
~
XXLG
fGalI
t
t
t xI
? Gal
t
t
Xyl Xyl
f
Xyl
Fuc
Xyl ~
XXXGXXXG
Xyl
t
XLXG
7 1 '
x
Xyl Xyl
t
G1c-t Glc-tG b+G Ic-t Gk+G Ic-tG Ic+G Ic Xyl Xyl
7 Gal
Glc+Glc+G k+Glc Xyl
t
J
XG8
t xI
Xyl
t
Ara
Glc+Gb+Glc-tGb
2-
s
3 v) P) c) c)
8
Xyl Xyl
7 7
s
e5
GIc+G Ic-tG Ic-t GIc-Gc-tG I c j GIc-t Glc
t
.z
3
1'
t t xI xI
2.
%
8
GlcjGlc
I 7 Gal
Glc-tGlc-tGlc+Glc Xyl
XXG
t
t
1
t
t
Xyl
Xyl Xyl
t
Xyl
t
New
XG7-01 XXXGol
Glc+Glc+Glc
GIc+G Ic-t GIc-tGlc Xyl
Gb+Glc+Glc+Glucitol
t
Fuc
t
Old
Structure
Xyl Xyl
f 7 Gal Gal t
7
Abbreviations
~
FIGURE 21 Abbreviated nomenclature of some xyloglucan oligosaccharides. (From Ref. 66.)
XXFGAXXG
lshii and Shimizu
200 a-L-Fucp 1
(1)
1 2 @D-Galp 1 I
I
FIGURE 22 Structure of xyloglucan repeating units of (1) XXFG and (2) XXXG.
wall would probably limit the self-association of cellulose fibers and might provide sites for cross-linking of cellulose fibers [64]. Xyloglucan appears to havea regulatory function as well asstructuralfunctions [7,64,65]. Xyloglucan oligosaccharides (XXFG) inhibited auxin-induced elongation of pea stem segments at about 10” M [78,79]. Related oligosaccharides lacking a fucosyl residue (XXLG and XXXG) are ineffectual. Xyloglucan oligosaccharides can promote the elongation of pea stem segments in the absence of 2,4-D [80].
/
OCH,
OH
OH
FIGURE 23 Structure of a feruloyl xyloglucan disaccharide.
201
Chemistry of Cell Wall Polysaccharides
f
1,11
Cellulose Microfibril FIGURE 24
Hydrogen bonds between cellulose microfibril
and xyloglucan. (From Ref. 64.)
C . Xylans Xylans are major hemicelluloses in the primary cell wall of monocots and are found in smaller amounts in the primary cell walls of dicots. Secondary walls of dicotyledonous plants contain a significant amount of xylan. The basic structure of xylan has been reviewed [4]. Xylans have a backbone of /3-1,4-linked xylose residues (Fig. 25). The backbone is substituted by varioussidechainsattachedthrough 0 - 2 or 0-3 of the xylosyl residues. Terminal arabinofuranosyl residues are usually attached to 0-3 of the 4-linked xylosyl residues. The backbone is substituted by a-linked 4-O-methyl-/3-~-glucopyranosyl uronic acid on 0 - 2 of xylosyl residues and acetyl esters on 0 - 2 or 0-3. The degree of side-chain substitution determines the degree of solubility of the xylan and its ability to bind to cellulose. Xylans having a high degree of side chains are more water soluble and bind less tightly to cellulose, whereas molecules with fewer side chains are less water soluble and bind to cellulose tightly. Primary cell walls of gramineous monocots contain esterified ferulic and p-coumaric acids [S l]. Three feruloyl and two p-coumaroyl arabinoxylan oligosaccharides were isolated from bamboo shoot cell walls (Fig. 26) [76,82-841. Feruloylation and p-coumaroylation occur at 0 - 5 of the arabinofuranosyl side chain of xylan. It has been hypothesized that the feruloyl esters are subjected to peroxidase-catalyzed coupling (Fig. 27) to yield a diferuloyl group, thereby cross-linking the xylan molecules. Such “lateral” cross-linking of polysaccharides could have profound effects on the physical properties of the cell wall and thus on its ability to grow and to resist enzymatic digestion [28,81]. Feruloyl arabinoxylan oligosaccharides appear to have regulatory functions just like xyloglucan oligosaccharides. The feruloyl oligosaccharides inhibited auxin-stimulated and gibberellin-inducedelongationgrowth of rice cells[85,86]. An arabinoxylanoligosaccharide has no inhibitory effect. Ferulic acid itself has weak inhibitory effect. These results indicate that the feruloyl substituent of feruloyl oligosaccharides is necessary for the inhibitory effect, but the glycosyl portion of feruloyl oligosaccharide is also important for increasing this inhibitory activity.
202
lshii and Shimizu
UH
OH
I
OH
H *' CH,O
0
A-
(3)
FIGURE 26 Structure of feruloyl and p-coumaroyl arabinoxylan oligosaccharides obtained from bamboo shoot.
D. p-1,3- and p-lY4-Glucan (P-Glucans) The p-glucans are important cell wall components in monocots. The P-glucans consist almost entirely of p-1,3- and P-1,4-linked D-glucopyranosyl residues. The ratio of p-1,3top-1,4-links is between 1:2 and 1:3 [5,30].The usualarrangementoflinkages is for single 1,3-linked residuestoseparatesequences of two, three, orfour 1,4-linked residues.
203
Chemistry of Cell Wall Polysaccharides
OH
FIGURE 26
Continued
E. Glucomannans Glucomannans are major hemicelluloses of the secondary cell walls of gymnosperms, as well as being a minor component of angiosperm secondary walls. This has beenwell summarized in the reviews [2-41.
VII.
A.
CROSS-LINKS BETWEEN CELL WALL POLYMERS
Covalent Linkages
1. GlycosidicLinkage There is Some evidence for covalent bonding between xylan and pectin. Kat0 and Nevins isolated arabinoxylan-rhamnogalacturonancomplex from maize cell walls [881.
h)
0 P
Polysaccharide
I Polysaccharide I
P 2H20
H202
Peroxidase H&O
Ferulate
Diferulate
OH
0
I
i ‘0
Polysaccharide
FIGURE 27
Formation of diferulic acid cross-link between polysaccharides. nl
3 P
Chemistry of Cell Wall Polysaccharides TABLE 8
Some Possible Cross-Links Between
205 Wall Polymers Cleaving reagents stated)(aq. unless
mple Possible Cross-link
(a) Covalent Glycosidic
Ester (uronoyl) Borate di-ester Ester (uronoyl, etc.)
Phenolic coupling (1) Ether (2) Biphenyl
Ether Disulfide (b)Noncovalent Hydrogen bond
Ionic bond
Arabinogalactan .RC-I Xylan. xyloglucan Xylan. RC Pectin. cellulose RC-II'RG-I1 Feruloyl .pectin Feruloyl .arabinoxylan Feruloyl . xyloglucan ( 1) Extensin. (Tyr-Tyr) . extensin (2) Pectinpectin Xyloglucan * xyloglucan Arabinoxylan arabinoxylan PS. (ether). feruloyl-PS Cystine (R-SS-R') Hemicellulose. cellulose
Extensin. pectin
Calcium bridge
Hydrophobic interaction van der Waals bonds Lectin bond
Gelling of pectin (also involves H-bonds) (Many) Lectin. PS
Endoglycanases, hot acid, dry HF
Esterases, Na,CO,, NaOH, MeOH/NaOMe Weak acid Esterases, NaOH, MeOWNaOMe
NaCIOz a pH 4 and 70°C (diferulate also cleaved by NaOH, etc.)
NaC102?BBr,? Dithiothreitol, mercaptoethanol MMNO, KOH (urea, guanidinium thiocyanate, and heat are not very effective) Salts (LaCI, > CaClz > NaCI), acids, alkalis Chelating reagents, e.g., EGTA, CDTA, EDTA, oxalate, hexametaphosphate; low pH Organic solvents (Reagents that change molecular conformation?) Sugar hapten; denaturation
Abbr-evrattorls: Ara, arabinose; Fer, ferulate;Gal,galactose;Glc,glucose, Me, methyl;MeOH,methanol; NaOMe, sodium methoxlde; PS, polysaccharide; RG-I, rhamnogalacturonan-I; Rha, rhamnose; Tyr, tyrosine. Source: Modified from Ref. 28.
2. Diferuloyl Cross-Link The occurrence of ferulic and p-coumaric acids ester-linked to arabinoxylans in grasses [87], to pectic polysaccharides in spinach [39-411 and sugar beet [40], and to xyloglucan in bambooshoot [76] is well characterizedasdescribed in the previous section. The possibility of covalent linkages betweenesterified ferulic acid on wall polysaccharides was first proposed in 1971 by Geissman and Neukon [89]. The ferulic acid residues on feruloyl arabinoxylan from wheat flour have been cross-linked with peroxidase and hydrogen peroxidase to make a gel. This demonstrated that a dehydrogenative coupling between two esterified ferulic acid residues on arabinoxylan to form dehydrodiferulic acid had occurred (Fig. 27). Sugar beet pectin that contains ferulic acid esterified to arabinose and galactose residues [40] also make gel following peroxidase-catalyzed, oxidative cross-linking [90].
lshii and Shimizu
206
The phenolic coupling has been invoked to explain termination of cell expansion. Small amounts of diferulate have been detected by alkaline hydrolysis of cell walls. The goal of detecting an oligosaccharide fragment, cross-linked by a diferuloyl bridge, was achieved in 1991 [91]. The linkage group was isolated and characterized from bamboo shoot arabinoxylan, providing definitive evidence for the existence of diferuloyl ester cross-link (Fig. 28). Ralph et al. [92] isolated a series of ferulic acid dehydrodimers in addition to 5-5 coupled dehydrodiferulate from saponified grass cell walls (Fig. 29). These dehydrodimers (8-5, 8-0-4, and 8-8) also are involved in cross-linking of polysaccharides in cell walls. Isolation ofwallfragmentscontainingthesedehydrodimers is animportant challenge. Other possibilities for dimerization of phenolic acid substituents of polysaccharides exist. A series of homo- and heterocyclodimers of the cyclobutane type, formed by headto-tail or head-to-head association of ester-linked p-coumaric acid and ferulic acids, were isolated [93] (Fig. 30). A similar peroxidase-catalyzed cross-link may occur between tyrosine residues of extensin (Fig. 31). The phenolic ether linkage of isotyrosine is known to form intramolecularly within extensin, and may also occur intermolecularly [28].
3. Ester Bonds Cold Na2C03,which hydrolyzes ester bonds but does not cause p elimination-degradation, solubilized pectin that is not solubilized by chelatingreagent or EPC [9]. Theseester bonds may be methyl esterified galacturonosyl residues, diferuloyl bridges, or ester bonds between uronic acids and neutral sugars. Although intermolecular ester bonds have been proposed [94], their identification has not yet been achieved.
4. Borate Diol-Diester Cross-Linkage Borate cross-links two RC-I1 molecules in pectic polysaccharide to form an RG-I1 dimer (Fig. 16). This cross-link is extremely acid-labile. Treatment of the borate-RG-I1 complex with 0.5 N HCl at room temperature for 30 min cleaved the borate ester linkage. The borate cross-linkage might play an important role in connecting pectin networks in the cell wall and may be involved in the acid-induced elongation of cells during growth.
"
O
H
c=C-C-OH 11
5 ) - a - ~ - A r a f -(1+3 ) -p-D-xylp- ( 1 4) -D-xylp
0
YCO
FIGURE 28 A diferuloyl arabinoxylan hexasaccharide isolated from bamboo shoot cell walls.
Chemistry of Cell Wall Polysaccharides
HOv
207
0
“ O v O OH
M S 0
FIGURE 29
B.
Structure of dehydrodimers of ferulates.
NoncovalentLinkages
As cell wall polysaccharides are polyhydroxylic, many hydrogen bonds form in the walls. Multiple hydrogen bondsare present within cellulose microfibrils. Hydrogen bondsare probably responsible for the incorporation of xylan, xyloglucan, and glucomannan into the cell wall. The hydrogen bonding between cellulose and xyloglucan, and between cellulose and xylan, has been demonstrated in vitro. Ionicbonds will be formed in the case of polymers that contain charged groups. Homogalacturonan and 4-O-methylglucuronoxylan have negative charges, while extensin has a positive charge. Ionic binding may occur between these charged polymers in the wall. Negatively charged galacturonic acid residues in homogalacturonan and RG-I can form cross-linking with Ca’+ to form an “egg-box” [95]. About 15-20 contiguousga-
lshii and Shimizu
208
OH
H0
FIGURE 30 Structure of cyclodimer of ferulic acid.
lacturonic acid residues are needed in each chain to make a stable complex. Methyl esterification in homogalacturonan and rhamnosyl residues in RG-I interrupt the concerted binding.Furthermore, acetylation occurs at 0 - 3 of galacturonicacidresidues in homogalacturonan [333 and at 0-2 and 0-3 of galacturonic acid residues of RG-I, respectively [35-371. Therefore,egg-boxcross-linkage is likely to be limited in the wall, although isolated pectin and pectin in jam and jellies are known to give rise to gel-like structures in vitro.
VIII.
CELL WALL MODEL OF GROWING PLANT CELL
The cell wall has a variety of components that assemble to form an extremely complicated structure. Several wall models have been proposed. An early cell wall model was proposed by Albersheim and co-workers [96]. This model contained covalent links between xyloglucan and RG-I and hydrogen bonds between cellulose and xyloglucan, leadingto indirect cross-linking of cellulose microfibrils through a series of hydrogen bonds and covalent bonds in the matrix. Some of the details of this model have been disproven by subsequent chemical analysis [ 181. Capita and Gibeaut [97] and McCann and Robert [98] have proposed structural models for primary cell walls basedon this new information. It is probably impossible to describe all cell wall components and their interactions with a single and simple model. However, the existence of two principal polysaccharide networks in the growing cell wall have been proposed: a tension-resistant load-bearing cellulose/xyloglucan network and a compression-resistant pectic polysaccharide network.
IX.
CONCLUDING REMARKS
Thischapter briefly summarizespresentknowledgeof the pectic polysaccharidesand hemicelluloses. Primary cell walls commonly contain cellulose, xyloglucan, arabinoxylan, homogalacturonan, RG-I, and RG-11. These six polysaccharides account for all or nearly all of the primary wall polysaccharides, and their primary structures have been well conserved among species. The six polysaccharides are to some extent cross-linkedby covalent and noncovalent bonds, making up a complicated macromolecular network in the primary
Chemistry of Cell Wall Polysaccharides
+
e e,
e, D
0
rc
209
lshii and Shimizu
210
walls. This chapter also discusses the functions of primary cell walls. The recent discovery that oligosaccharide fragments derived from cell wall polymers in growing tissues can act as potent and specific regulators of gene expression is of importance to the biochemistry of all living systems [see refs. 34,99,100].
REFERENCES 1. 2. 3. 4.
5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19.
G. 0. Aspinal, Advan. Carbohyd,: Chem., 14: 429 (1959). T. E. Timell, Advan. Carbohyd,: Chem., 19: 247 (1964). T. E. Timell, Advan. Carbohydr: Chem., 20: 409 (1965). K. Shimizu, in Wood and Cellulosic Chemistry (D. N.-S. Hon and N. Shiraishi, eds.), Marcel Dekker, New York, p. 177 (1991). A. G.Darvill, M. McNeil, P. Albersheim, and D. P. Delmer, in The Biochemistry ofplants, 1 (N. E. Tolbert, ed.), Academic Press, New York, p. 91 (1980). P. Albersheim and A. G. Darvill, Sci. Am., 253(3):58 (1985). M. McNeil, A. G. Darvill, S. C. Fry, and P. Albersheim, Ann. Rev. Biochem., 53: 625 (1984). J. R. Thomas, M. McNeil, A. G. Darvill, and P. Albersheim, Plant Physiol., 83: 659 (1987). M. A. O’Neill, A. G. Darvill, and P. Albersheim, Methods Plant Biochem., 2: 415 (1990). B. W. Simson and T. E. Timell, Cellulose Chem. Technol., 12: 39 (1978). B. W. Simson and T. E. Timell, Cellulose Chem. Technol., 12: 51 (1978). B. W. Simson and T. E. Timell, Cellulose Chem. Technol., 12: 63 (1978). B. W. Simson and T. E. Timell, Cellulose Chem. Technol., 12: 79 (1978). B. W. Simson and T. E. Timell, Cellulose Chem. Technol., 12: 137 (1978). Y. Edashige, T. Ishii, T. Hiroi, and T. Fujii, Hol~orchung,49: 197 (1995). W. S. York, A. G. Darvill, M. McNeil, T. T. Stevenson, and P. Albersheim, Methods Erzzymol., 118: 3 (1986). R. R. Selvendran and M. A. O’Neill, Methods Biochem. Anal., 118: 3 (1986). P. M. Dey and K. Brinson, Advan. Carbohyd,: Chem. Biochem., 42: 265 (1987). C. Brettand K. Weldron,in Topics in PlantPhysiology, 2, Unwin Hyman, London, p. 4 ( 1990).
20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30. 31. 32. 33. 34.
35. 36.
G. 0. Aspinal, in Techniques of Chemistry, 4 (K. W. Bentley and G. W. Kirly, eds.), WileyInterscience, New York, p. 379 (1973). P. Albersheim, D. J. Nevins, P. D. English, and A. Karr, Carbohyd,: Res., 5: 340 (1967). S. Hakomori, J. Biochem. (Tokyo), 55: 205 (1964). A. G. Darvill, M. McNeil, and P. Albersheim, Plant Physiol., 62: 418 (1978). A. B. Blakeney and B. A. Stone, Carbohyd,: Res., 140: 3 19 (1985). I. Ciucanu and F. Kerek, Carbohydr: Res., 133: 105 (1984). A. Isogai, A. Ishizu, J. Nakano, S. Eda, and K. Kato, Carbohyd,: Res., 138: 99 (1985). P.-E. Jansson, L. Kenne, H. Liedgren, B. Lindberg, and J. Lonngren, Chern. Commun. Univ. Stockholm, No. 8 ( 1976). S. C . Fry, Ann. Rev. Plant Physiol., 37: 165 (1986). X. Qi, B. X. Behrens, P. R. West, and A. J. Mort, Plant Physiol., 108: 169 1 ( 1995). A. Bacic, P. J. Harris, and B. A. Stone, in Biochemistry of Plunts, 13 (J. Preiss, ed.), Academic Press, San Diego, CA, p. 297 (1988). E. Nothnagel, M. McNeil, and P. Albersheim, Plunt Physiol., 71: 916 (1983). G. 0. Aspinal, Polysaccharides, Pergaman Press, Oxford, U.K. (1970). T. Ishii, Plant Physiol., 113: 1265 (1997). A. Darvill, C. Auger, C. Bergmann, R. W. Carlson, J.-J. Cheng, S. Eberhard, M. G. Hahn, V.-M. L6, V. Marfi, B. Meyer, D. Mohnen, M. A. O’Neill, M. D. Spiro, H. van Halbeek, W. S. York, and P. Albersheim, Glycobiology,2: 181 (1992). P. Komalarilas and A. Mort, Curbohydr: Res., 189, 261 (1989). P. Lerouge, M. O’Neill, A. G. Darvill, and P. Albersheim. Cnrbohyd,: Res., 243, 359 (1993).
Chemistry of Cell Wall Polysaccharides
37. 38. 39. 40. 41. 42.
211
T. Ishii, Mokuzui Gakkuishi, 41, 561 (1995). Y. Edashige and T. Ishii, Phytochemistry, 42, 61 1 (1996). S. C . Fry, Biochem. J., 203, 493 (1982). T. Ishii, Plant Cell Physiol., 35, 701 (1994). T.Ishii and T. Tobita, Carbohyd,: Res., 248, 179 (1993). M. W. Spellman, M. McNeil, A. G. Darvill, P. Albersheim, and K. Henrick, Carbohydr. Res.,
122, 115(1983). 43. A. J . Whitcome, M. A. O’Neill, W. Steffan, P. Albersheim,and A. G. Darvill, Curbohyd,: Res., 271, 15 (1995). 44. V. Puvanesarajah, A. G. Darvill, and P. Albersheim, Curbohyd,: Res., 218, 21 1 (1991). 45. J. T. Thomas, A. G. Darvill, and P. Albersheim, Curbohydr. Res., 185, 261 (1989). 46. T. T. Stevenson, A. G. Darvill, and P. Albersheim, Curbohyd,: Res., 182, 207 (1988). J. Brasch, Curbohyd,: Res., 209, 191 (1991). 47. R. J . Regwell, L. D. Melton, and D. 48. T. Ishii, Mokuzui Gukkaishi, 41, 669 (1995). 49. M. Kobayashi, T. Matoh, and J. Azuma, Plant Physiol., 110, 1017 (1996). 50. T. Ishii and T. Matsunaga, Curbohydr. Res., 284, 1 (1 996). P. Pellerin, T. Doco, A. G. Darvill, and P. Alber51. M. A. O’Neill, D. Warrenfeltz, K. Kates, sheim, J. Biol. Chem., 271, 22923 (1996). Phytochemistry, 44, 243 (1997). 52. S. Kaneko, T. Ishii, and T. Matsunaga, 53. B. J. Shelp, in Boron and Its Role in Crop Production (U. C. Gupta, ed.), CRC Press, Boca Raton, FL, p. 58 ( 1992). 54. W. D. Loomos and R. W. Durst, Bio Factor, 3, 229 (1992). 55. H. 0. Bouveng, Acta Chem. Scand., 19, 953 (1965). G. J. Voragen, Carbohyd,: Res., 279, 265 56. H. A.Schols,E. J. Bakx,D.Schipper,andA. (1995). 57. I. Eriksson, R. Andersson, E. Westerlund, R. Andersson, and P. Aman, Curbohyd,: Res., 281, 161 (1996). G. Darvill,and P. Albersheim, Curbohydr: Res., 243, 373 58. P. Lerouge,M.A.O’Neill,A. ( 1 993). 59. M. McNeil, A. G. Aman, and P. Albersheim, Plant Physiol., 70, 1586 (1982). 60. J. M. Lau, M. McNeil, A. G. Darvill, and P. Albersheim, Curbohyd,: Res., 168, 245 (1988). 61. S. Eda, K. Miyabe, Y. Akiyama, A. Ohnishi, and K. Kato, Curbohyd,: Res., 158, 205 (1986). 62. A. M. Stephen, in The Polysaccharides, 2 (G. 0. Aspinal, ed.), Academic Press, New York, p. 97 (1980). 63. H. Du, A. E. Clarke, and A. Bacic, Trends Cell Biol., 6, 413 (1996). 64. T. Hayashi, AIUIU.Rev. Plant Physiol. Plant Mol. Biol., 40, 139 (1989). 65. S. C. Fry, J. Exp. Bot., 40,1 ( 1989). 66. S. C.Fry, W. S. York,P.Albersheim,A. G. Darvill, T. Hayashi, J.-P. Joseleau, Y. Kato, E. P. Lorences, G. A. Maclachan, M. McNeil, A. J. Mort, J . S. Reid, H. U. Seitz, R. R. Selvendran, A. G. J. Voragen, and A. R. White, Physiol. Plant, 89: 1 (1993). 67. W. S. York, J . E. Oates, H. van Halbeek, A. G. Darvill, and P. Albersheim, Carbohyd,: Res., 173, 113 (1988). 68. L. L. Kiefer. W. S. York, A. G. Darvill, and P. Albersheim, Phytochemistry, 28: 2105 (1989). 69. L. L. Kiefer. W. S. York, P. Albersheim, and A. G. Darvill, Carbohyd,: Res., 197, 137 (1990). 70. M. Hisamatsu, G. Impallomeni, W. S. York,P.Albersheim,andA. G. Darvill, Curbohyd,: Res., 211, 117 (1991). 71. M. Hisamatsu, W. S. York. A. G. Darvill, and P. Albersheim, Carbohyd,: Res., 227.45 (1992). 72. W. S. York,H.vanHalbeek,A. G. Darvill,and P. Albersheim. Carbohyd,:Res., 200. 9 (1990). 73. W. S. York, G. Impallomeni,M.Hisamatsu, P. Albersheim,andA. G. Darvill, Carbohyd,: Res., 267, 79 ( 1995). 74. W. S. York. V. S. K.Kolli, R. Orlando, P. Albersheim, and A. G. Darvill, Cur-bohydr. Res., 285. 99 (1996).
212
lshii and Shimizu
75. 76. 77. 78. 79. 80. 81.
T. Ishii, J . R. Thomas, and T. Hiroi. Phytocher,~i.st~~, 29: 1999 (1990). T. Ishii and T. Hiroi, Curbohyrlr. Res., 206, 297 (1990). S. Aldington, G. J. McDougall, and S. C. Fry, Plant Cell, u r d Enr~iromnent,14: 625 (1991). W. S. York, A. G. Darvill, and P. Albersheim, Plant Physiol., 75: 295 (1984). G. J. McDougall and S. C . Fry, Plmta, 175: 412 (1988). G. J . McDougall and S. C . Fry, Plant Physiol., 93: 1042 (1990). J. Ralph and R. F. Helm, in Foruge Cell Wull Structure und Digestibility (H. G. Jung, D. R. Buxton, R. D. Hatfield, and J. Ralph, eds.), American Society of Agronomy, Madison, WI, p. 201 (1993). T. Ishii and T. Hiroi, Crrrbohydr: Res., 196: 175 (1990). T. Ishii, Phytochetnistry, 30: 23 17 (1991). T. Ishii, Mokrczai Cakkuishi, 42: S15 (1996). T. Ishii and H. Saka, Pltrnt Cell Physiol., 33: 321 (1992). T. Ishii and T. Nishijima, Plant Cell Physiol., 36: 1447 (1995). K. Iiyama, T. B.-T. Lam, and B. A. Stone, Plunt Physiol., 104: 3 IS (1994). Y. Kato and D. J. Nevins, Curbohydr: Res., 227: 315 (1992). T. Gerssman and H. Neukom, Helv. Chern. Acttr, 54: I108 (1971). F. M. Rombouts, J. F. Thibault, and C. Mercier, French Patent Appl. 83,07,208; Chern. Abstt;
82. 83. 84. 85.
86. 87. 88. 89. 90.
102: 60792u (1983). 91. T. Ishii, Curbohydr. Res., 21 9: IS ( 1 991). 92. J. Ralph. S. Quideau. J . H. Grabber, and R. D. Hatfield, J . Chern. Soc. Perkin Truns.. I : 3485 ( 1994). 93. W. H. Morrison, 111. R. D. Hartley, and D. S. Himmelsbach. J. Agric. Food Chem., 40: 766 ( 1992). 94. J. A. Brown and S. C. Fry, Plont Physiol., 103, 993 (1993). 95. D. A. Powell, E. R. Morris, M. J. Gidley, and D. A. Rees, J . Mol. Biol.. 155: 5 17 (1982). 96. P. Albersheim, M . Rev. Bioc.hern., 16: 127 (1978). 97. N. C. Carptia and D. M. Gibeaut, Plont J., 3: 1 (1993). 98. M. C . McCann and K. Roberts, J . Exp. Bot., 45. 1683 ( 1994). 99. S. A. Ldington and S. C. Fry, A h . Bot. Res., 19: I (1993). 100. F. CBte and M. G. Hahn, Plunt Mol. R i o / . , 26: 1379 ( 1994).
Chemistry of Extractives Toshiaki Umezawa Kyoto University, Kyoto, Japan
1.
INTRODUCTION
Extractives are the wood constituents which can be extracted with neutral solvents. They are obtained by extracting wood meal with organic solvents or water or by steam distillation, and some are obtained as exudates from wounded trees. The amountofextractives is small,generallyupto 5-10% in the woodin the temperate zone. However, in some tropical woods relatively high amounts of extractives are found [l]. Amongwood species, differences of chemical structures of three major cell wall components, cellulose, hemicellulose, and lignin, are few. However, a great diversity in extractive composition is found throughout wood species. Although the extractives are low in concentration compared with those of the cell wall polymers, this fraction characterizes eachwoodspecieschemically.Mostcomponents of woodextractives are classified as secondary metabolites, and the distribution of specific compounds is restricted in certain wood species. This feature provides the basis of chemotaxonomy of woody plants. Furthermore, individual compounds are often found in specific tissues of individual trees, and their amounts can vary from season to season even in the same tissue. Many phenolic compounds are accumulated in heartwood, whereas they are found only in trace amounts in the corresponding sapwood. Extractives are the predominant contributors to woodcolor, fragrance, and durability. Extractives also influencethe pulping, drying, adhesion, hygroscopicity, and acoustic properties of wood.Manyextractiveshave specific biological activities, andvariouswoods have been used as sources of crude drugs and medicines for centuries. Recent progress of the biosynthesis of secondary metabolites of woody plants including heartwood components [2] has suggested the possibility of biotechnological control of their biosynthesis. This may lead to biotechnological production of biologically active extractives, and to elucidating molecular mechanisms of heartwood formation. Progress in the chemistry and biochemistry of natural products including wood extractives has been reviewed in a number of articles, such as in Natural Product Reports. Thisjournalincludesregularreviews of the relevant literature publishedduringwelldefined periods with respect to individual topics in the fields.
213
214
Umezawa
II. LIGNANS, NEOLIGNANS, AND RELATED COMPOUNDS Lignans and neolignans are phenylpropanoids that occur in many plants including softwoods, hardwoods, and medicinal plants [3-51. The term “lignan” was introduced by Haworth to describe a group of phenylpropanoid dimers, where the phenylpropane units were linked by the central carbon (C8) of their side chains [6]. Gottlieb coined “neolignan” for compounds containing two phenylpropane units that are linked otherwise than C8-C8’ [7]. Later, neolignans were redefined as the dimers of allyl- or propenylphenyls, while lignans were regarded as the dimers of cinnamyl alcohols [8]. However, in this review Haworth’s definition of lignans [6] and Gottlieb’s former definition of neolignans [7] will be used, because the original definitions are being applied by most researchers. Tri- and tetramers of phenylpropanoid units are referred to as sesqui- and dilignans, respectively. Lignans are classified into several subgroups:dibenzylbutanes,dibenzylbutyrolactones, furans, furofurans, aryltetralins, arylnaphthalenes, and dibenzocyclooctadienes [3,5] (Fig. I). Lignans often occur as glycosides. Examples of neolignans are shown in Fig. 2. Chemical structures of lignans and neolignans are similar to that of lignins. Thus (+)-pinoresin01 (5) and the corresponding (-)-enantiomer are typical lignans, while this structure is also involved in a lignin molecule as a substructure (i.e., pinoresinol or p-p’ substructure) [9]. Also the structures of neolignans are similar to lignin substructures of p-0-4 (arylglycerol p-aryl ether), 5-5’ (biphenyl), and p-5 (phenylcoumaran) types [IO]. In spite of the structural similarities, lignins differ sharply from lignans and neolignans in terms of optical activity. The former is optically inactive, while the latter is optically active, suggesting the difference in stereochemical mechanisms in their biosyntheses [9]. Following the first example of an in-vitro enantioselective formation of an optically pure lignan, (-)-secoisolariciresinol (l),with an enzyme preparation from Forsythia inin lignan biosynthesis termedia [ 1 l], much investigation has been done for enzyme systems of Forsythia spp. [9,12,13]. Figure 3a shows the conversion of coniferyl alcohol (14) into lignans with Forsythia enzymes. Recently, cDNA cloning of pinoresinol/lariciresinol reductase which catalyzes reduction of (+)-pinoresin01 (5) and (+)-lariciresinol (4) to (+)lariciresinol (4) and (-)-secoisolariciresinol (l),respectively, has been reported [ 141. In addition, enantioselective coupling of two coniferyl alcohol radicals giving rise to (+)pinoresinol (S) was reported [15]. The coupling was highly enantioselective only in the presence of dirigent protein isolated from Forsythia plant. Formation of (+)-secoisolariciresinol (lS), the oppositeenantiomerto the one in Forsythia spp.,with an enzyme preparation from Arcfiurn lappa petioles, has been reported (Fig. 3b) [16]. On the other hand, an enzyme preparation from seeds of A. lappa was recently found to catalyze enantioselective formation of (-)-secoisolariciresinol (1) from coniferyl alcohol (14), indicating that two enzyme preparations from different organs of a single plant species can catalyze the selective formation of different enantiomers of a lignan [ 171. The structural similarity with lignins suggests that neolignans maybe synthesized by enantioselective coupling of two phenolic phenylpropane units. Recently, two examples of enantioselectiveformation of neolignansfrom coniferyl alcohol (14) werereported [18,191. Lignanshavesuch biological activities asantitumor[podophyllotoxin (7) and steganacin (9)], antimitotic [podophyllotoxin (7)],antioxidant (nordihydroguaiaretic acid andsesaminol), and antiviral [podophyllotoxin (7) againstcytomegalovirusandherpes simplex l-virus, and (-)-arctigenin (3) against human immunodeficiency virus], etc. [3-
215
Chemistry of Extractives
Furan
Dibenzylbutane Dibenzylbutyrolactone
OH
H0 OCH3 -Secoisolariciresinol (-)
1
R=E (-) "atairesinol 2 Re83 (-) -Arctigenin 3
Aryltetralin
E'urofuran
OCH3
OCH3 R=E (+) -Pinoresin01 5
Podophyllotoxin 7
R=OC83 (+) -Syringaresinol 6
DibenzocycloGlycoside octadiene
Steganacin 9 FIGURE 1
Arctiin
10
Examples of lignans.
OCH3
Kadsurenone 11 FIGURE 2
(+) -Lariciresinol 4
Magnololl2 Eonokiol13
Examplcs o f neolignans.
Diphyllin
8
Umezawa
216
%" Coniferyl alcohol 14
(+) -Pinoresinol 5
(+) -Larici-
I
J
(-) -Secoisolariciresinol resinol 1
(-) "atai2
(-)
resinol 4
--ct
igenin 3
(b)
H3CO H O T : :
OCH3 Coniferyl OH
alcohol 14
\
0
OH
O C H ~ (+) -Secoisolariciresinoll5
FIGURE 3 Enzymatic lignan formation.
5,201. Antagonism toward the platelet-activating factor (veraguensin) and inhibitory activities toward certain enzymes have also been detected in many lignans [3-5,201. Among the biologically active lignans, antitumor podophyllotoxin (7)has attracted particular interest [see also Section XLC]. Mammalian lignans are known to be produced from plant lignans such as secoisolariciresinol diglucoside by the action of bacterial flora in the colon of human or animals. The mammalian lignans and their precursor secoisolariciresinol diglucoside have a protective effect on the promotion stage of mammary tumorigenesis [21], and are receiving widespread interest. A neolignan, kadsurenone (ll),has antagonistic activity to platelet-activating factor [22].Honokiol (13) is antibacterial and antifungal, and magnolol (12) has antimicrobial and muscle-relaxant activities [23,241.
111.
NORLIGNANS
Norlignans are diphenylpentane (C,-C,)-(Cz-C,) compounds, and typical examples are shown in Fig. 4. Although the biosynthetic sequences for norlignans have not been elucidated, the structures are seemingly composed of the phenylpropane (C,-C,) and phen-
217
Chemistry of Extractives
OH
Hinokiresinol 16
Sequirin (Sequirin-C) 18
Agatharesinol 17
Sugiresinol Hydroxysugiresinol Cryptoresinol (Sequirin-B) 20
21
( Sequirin-A) 19
HdHaWO H0 OH
Pueroside-A OH 22
H O f/l o H
cis-Hinokiresinol 23
\3
OH
Yateresinol Sequirin-D nyl)-2-cyclo-pentene24 25 FIGURE 4
2,3-Bis(p-hydroxy-phe l-one 26
Examples of norlignans.
ylethane (C,-C,) units connected via C8-C7' [e.g., hinokiresinol (16)] and in some cases C8-C8' [e.g., yateresinol (24)] and C9-C8' [e.g., sequirin-D (25)](Fig. 4). Most norlignans have been isolated from softwoods belonging to Cupressaceae, Taxodiaceae, and Araucariaceae [25-271, while some norlignans occur in herbaceous plants. cis-Hinokiresinol (23) was isolated from Anen7arrl1et~a crspI7ndt.loide.s (Liliaceae) 1281, and two norlignan glycosides, pueroside-A (22) and -B, were isolated from PuercrriLI lohtc1 (Leguminosae) [29] (Fig. 4). No concrete experimental evidence has been reported for the origin of the two aromatic nuclei of a norlignan molecule. Based on structural considerations, several possible schemes have been proposed for the biosynthesis of norlignans, involving coupling of two phenylpropane units followed by loss of one carbon atom 125,301. Norlignans are of particular interest with respect to heartwood coloration. The coloration of heartwood of Japanese cedar (Cty>tornc~ria japonica) is due to polymerization
Umezawa
218
of norlignans, e.g., hydroxysugiresinol (20) and sequirin-C (18) [31,32], andthat of hinoki cypress (Charnaecyparis obtusa) is related to hinokiresinol (16) [33]. Inhibitory activity on cyclic adenosine-3’,5’-monophosphatephosphodiesterase was reported for cis-hinoki resinol (23) [28]. Sugiresinol (19) and hydroxysugiresinol (20) have inhibitory effect on polymerization of methyl methacrylate [34].
IV.
FLAVONOIDS
Flavonoids are diphenylpropane (C,-C&,) compoundswhicharecomposedof the C,-C, (phenylpropane) fragment derived from the shikimate-cinnamate pathway and the C , fragmentderivedfrommalonyl-CoA (40). Flavonoids are classified into flavanones, flavones, chalcones, dihydroflavonols (flavanonols), flavonols, aurones, flavan-3-01s (catechins), flavan-3,4-diols (leucoanthocyanidins),anthocyanidins, isoflavonoids, andneoflavonoids (Fig. 5). The term “flavonoids” in the strict sense is sometimes applied to those except for isoflavonoidsandneoflavonoids.Proanthocyanidins(condensedtannins) are oligomers and polymers of polyhydroxyflavan-3-01 units [35] (see also Section IX). Typical examples of flavonoids are shown in Fig. 5. Flavonoids occur widely in the plant kingdom, and presentwidelyor specifically in barks, heartwoods, flowers, fruits, seeds, roots, etc. Flavonoids reported to occur in wood or bark are listed in Ref. [36], and the chemistry of flavonoids is reviewed in a number of works [36-411. Chalcone is biosynthesizedfromcinnamoyl-CoAs [especially, p-coumaroyl-CoA (39)], which is formed via the shikimate-cinnamatepathway,and three moleculesof malonyl-CoA (40). The transformation is catalyzed by chalcone synthase as shown in Fig. 6.6’-Deoxychalcone [e.g., isoliquiritigenin (30)] is likewisesynthesizedfrommalonylCoA (40) and 4-coumaroyl CoA (39) by chalcone synthase in coaction with a NADPHdependent polyketide reductase. The chalcones are the immediate precursors for all flavonoids (in the strict sense). Thechalcones are converted to flavanones, flavones, dihydroflavonols, flavonols, leucoanthocyanidins, anthocyanidins and their glycosides (anthocyanins), catechins, and aurones [42,43]. The enzymes which are responsible for these conversions and the genes encoding these enzymes have been well characterized [42,44481. Formation of isoflavonoidsinvolves the rearrangement of aphenylgroupof the flavanoneskeleton[42,46].On the otherhand, little is knownaboutbiosynthesisof neoflavonoids. Flavonoids have various biological activities 137,381. Thus, symbiotic nitrogen-fixing bacteria recognize flavonoids as signals for the activation of their nodulation genes [49]. Isoflavonoids are the major structural class of phytoalexins in legumes [49-511. Anthocyanins occur as flower pigments [52,53]. Green teas contain significant amounts of catechins which have an antioxidant activity [54]. The effects of flavonoids on mammalian biology are reviewed [55,56]. Flavonoids seem to protect plants from ultraviolet-induced injury 1571. Manyflavonoids are biosynthesized in response to externalstresses, e.g., ultraviolet light, microbial attack, and physical injury. Hence, the flavonoid biosynthesis is a metabolic event which is suitable to investigate stress-gene expression relation. Heartwood formation which does not occur in herbaceous plants is one of the metabolic events specific to woody plants, but little is known about its biochemical mechanisms. However, this metabolic event involves or is accompanied by deposition of significant amounts of secondary metabolites, so-called heartwood extractives suchas flavonoid, stilbene, lignan, norlignan, etc. Seasonal changes and site specificity of chalcone synthase activity have been examined in relation to heartwood flavonoid synthesis [58,59].
Chemistry of Extractives
219
Qfy
Flavanone
Cbalcone
Flavone
\
0
H OH 0 Sakuranetin 27
Dihydroflavonol (Flavanonol)
\
I OI
S
OH 0 Apigenin 28
H
O
\
R
S
0
R=on, Chalconaringenin 29 R=H, Isoliquiritigenin 30
Aurone
Flavonol
OH 0
H o e : : I
'
I
OH
OH 0
Dihydrokaempferol 31
Flavan-3-01 (Catechin)
Quercetin 32
OH
0
Sulfuretin 33
Flavan-3,I-diol (Leucoanthocyanidin) Anthocyanidin
OH
OH OH
H \o d : :
H o e OHo H
OH OH
(+)-Catechin 34
OH OH
Leucodelphinidin 35
Isoflavonoid
Neoflavonoid
% Daidzein 37
FIGURE 5 Examples of flavonoids.
OH Pelargonidin 36
Umezawa
220
p-Coumaroyl-CoA 39
Flavonoids
HOOC>SCoA
0 Malonyl-CoA 40 FIGURE 6 Biosynthesis of flavonoids and stilbenes.
Many genes of the enzymes involved in flavonoid synthesis have been cloned, and mechanisms of the gene expression have been investigated intensively [47,48]. Thus, flavonoids are one of the best-understood groups of plant secondary metabolites, especially in terms of biosynthesis. It should be noted that extensive genetic information available about flavonoids, especially anthocyanin pigments of flowers, has accelerated significantly the biosynthetic studies in this field.
STILBENES
V.
Historically, the termstilbene referred to compoundspossessing the 1,2-diphenylethene structure,butnowadays the newlydiscoveredbibenzylsandphenanthrenes,whichare composed of C,-C,-C, skeleton, are also involved in this group. Stilbenes occur in the Pinaceae, Moraceae, Betulaceae, Leguminosae, etc. [60]. Typical examples of this class are shown in Fig. 7. Stilbenes are elaborated from CoA esters of cinnamic acids, and there is a similarity in the biosynthesis of stilbenes with that of flavonoids (Fig. 6). Stilbene synthases catalyze
Resveratrol
Pinosylvin
Elydxangeic acid
42
I
OH
Lunularin
Batatasin I
45
FIGURE 7 Examples
or stilbenes.
Chemistry of Extractives
221
condensation of CoA estersof cinnamic acids [e.g., cinnamoyl-CoA and p-coumaroyl-CoA (39)J with three molecules of malonyl-CoA (40), as in chalcone synthesis catalyzed by chalcone synthase [2,61]. However, the cyclization of polyketide moiety of the C& polyketocarboxylic acid (41) occurs in a different wayfrom that by CHS to give rise to stilbenes (Fig. 6); resveratrol (42) and pinosylvin (43) are formed with elimination of one carbon atom (Fig. 6),while hydrangeic acid (44) is formed without the elimination [61,62]. Although pinosylvin (43) and pinosylvin monomethyl ether occur in sound heartwood of Pinus spp., they are formed as a response to stress such as fungal infections or UV light [601. Hence, the role of stilbene in decay resistance and induction of stilbene synthesis has attracted much attention [60]. A stilbene synthase from UV-stressed seedlings of Pinus sylvestris has been purified and characterized [63], while a stilbene synthase gene from grapevine (Vitis vintfera) was transferred to tobacco, and the regenerated plants were found to display increased resistance to Botrytis cinerea [64]. Pinosylvin (43) and pinosylvin monomethyl ether are also known as inhibitors of sulfite pulp cooking [65].
DIARYLHEPTANOIDS
VI.
Diarylheptanoids are composed of two phenyl rings connected with a C , carbon chain (Fig. 8). Many of this type of compound are isolated from plants belonging to the Betulaceae and Zingiberaceae. Besides these two families, the occurrence of diarylheptanoids in the following species was also reported: Centrolobium spp. (Leguminosae), Myrica spp. (Myricaceae), A c e r spp. (Aceraceae), and Garuga spp. (Burseraceae). Recently the chemistry and biological activity of diarylheptanoids have been reviewed [66,67].
OH OH
0 0
Ilannokinol 47
Curcumin 48
OH
H0
P l a t y p h y l l o s i d a 49 0
"'OH H 0 OH
Asadanin 50 FIGURE 8
Acerogenin
Examples of diarylheptanoids.
A 51
Urnezawa
222
Two different results of feeding experiments have been reported regarding biosynthetic precursors of diarylheptanoids. One suggested that one aromatic ring of curcumin (48) is derived from a cinnamate unit and the other from acetate (or malonate), based on administration of [ I4C]acetate, [I4C]malonate, and [14C]phenylalanine to Curcuma longa [68]. Other studies suggestedthat diarylheptanoids, acerogeninA (51), and platyphylloside (49) were derived from two phenylpropane units and one acetate (or malonate)unit, based on administration of [“C]cinnamate, [14C]phenylalanine, [ I4C]acetate, and [ 14C]malonate to Acer nikoense [acerogenin A (51)] [69], and of [14C]cinnamate and [I4C]malonate to Betula platyphylla [platyphylloside (49)] [70].
VII.
ISOPRENOIDS
lsoprenoids is the generic name of compounds composed of isoprene (C,H,) units connected linearly or cyclically. Isoprenoids consist of terpenoids, steroids, and tropolones. Since the chemistry of terpenoids, steroids, and tropolones has been developed independently in spite of their close relationship in biosynthesis, the three classes are usually treated separately. Terpenoids are divided into monoterpenes (C,,,), sesquiterpenes (C,,), diterpenes (C?”), sesterterpenes(C,,), triterpenes (C,,,), tetraterpenes (C,,), and polyterpenes (C,,,), depending on the number of the constituent isoprene (C,) units. Each subclass of terpenoids is further classified into many groups of different carbon skeletons. The terpenoid compounds are generally elaborated via the mevalonate pathway as outlined in Fig. 9. Although the mevalonate pathway has generally been accepted, a novel pathway concerning the early steps of isoprenoid biosynthesis toward isopentenyl pyrophosphate (56) has recently been demonstrated [71]. The novel pathway, which involves the condensation of a triose phosphate with activated acetaldehyde, has been characterized in several different bacteria [71,72]. In addition,Eisenreichetal.haveshown that the taxane carbon skeleton is not of mevalonate origin in Taxus chinensis [73] (see also Section X1.C). Isoprenoids are the largest group among plant secondary metabolites, and occur in a huge number of plants including woody plants. It is beyond the scope of this book to list all the plants producing this class of compounds and to describe their biosynthetic schemes. Comprehensive lists of the compounds, their biosynthesis, and biological activities are summarized elsewhere [2,37,74-771.
A.
Terpenoids
Specific fragrances of different woods are usually due to the composition of monoterpenes and volatile sesquiterpenes. They can be easily separated from wood by steam distillation, and the oily substance obtained is called “essential oil.” Turpentine, essential oil from Pinus spp., is obtained by steam distillation of exudates from pine trees (oleoresin); the residue is gumrosin,which is composedmainly of diterpene acids (rosin acids), e.g., abietic acid (91). Turpentines obtained from pine wood and those recovered from kraft pulp waste liquor are called wood turpentine and sulfate turpentine, respectively. Rosins are used for sizing of papers. Monoterpenes are derivedfromgeranylpyrophosphate (58). They are subdivided into acyclic and cyclic monoterpenes (Fig. IO) a-Pinene (64) and @-pinene (65) are major components of turpentine.
223
Chemistry of Extractives
y SCoA
y SCOA Acetyl-coA
Acetyl-coA 52
52
Ki,SCOA Acetoacetyl-coA 0 ,o
53
3-Eydro~y-3-methylglutaryl-CoA 54
Mevalonic
- JJPP
acid55
pyrophospxate 1 56
1
Isopenten
uopp
"-l l
Dimethylallyl pyrophosphate 57
I
OPP
Monoterpenoids
M Geran
1 pyropiosphate 58
Sesquiterpenoids Squalene \ TriFarnesyl pyrophosphate 59 terpenoids
'
.
Diterpenoids \ Tetraterpenoids c
G e r m lgeranyl 'Phytoene pyropxosphate 60
Sesterterpenoids Getan lfarnesyl pyropiosphate 61
Polyterpenoids FIGURE 9 Generalscheme of terpenoid biosynthesis. PP: pyrophosphategroup.
Sesquiterpenes are derived fromfarnesyl pyrophosphate (59), and constitute the largest class of terpenoids [74]. Some 120 distinct skeletal types of sesquiterpenes are known [74]. Figure 11 depicts the important sesquiterpene skeletal types from acyclic (e.g., farnesane) to tricyclic (e.g., thujopsane), which are often encountered as wood constituents. Qpical examples of each type of sesquiterpenes are also shown under the corresponding skeletal types in Fig. 11. Diterpenes are derived from geranylgeranyl pyrophosphate (60), and some 130 distinct skeletal types are reported [74]. Figure 12 shows the typical diterpene skeletal types
Urnezawa
224
P-Myrcene
(-) -Citronellol
62
63
(-) 64
-a-Pinene
(-) +-Pinene
65
(- ) -Limonene
1,B-Cineol
67
68
(+) -Camphor 66
FIGURE 10 Examples of monoterpenes.
with corresponding examples. A phytane diterpene, plaunotol (87), has anti-ulcer activities [78]. ent-Gibberellane diterpenes, gibberellins, are important plant hormones. Occurrence of sesterterpenes in higher plants is highly limited. Triterpenes are elaborated from squalene formed via tail-to-tail coupling (coupling between pyrophosphate ends) of two farnesyl pyrophosphate units 121. Two major classes of nonsteroidal triterpenes are tetracyclic and pentacyclic [74]. Examples of typical skeletal types of this class are shown in Fig. 13: lanostane, dammarane,euphane,limonoids [tetranor (C,,) compounds], quassinoids (mainly Czo compounds), lupane, and oleanane. Figure 13 also shows examples of compounds belonging to each skeletal type. Oleananes often occur as aglycons (sapogenins) of saponins [76].
B. Steroids Steroids, which are also derived from squalene, are compounds with cyclopentanoperhydrophenanthrene skeleton and their congeners elaborated from them. The basic structure of steroids is shown in Fig. 14. Positions on the same side as the angular methyl (18- and 19-CHJ are denoted as p, and those on the opposite side are denoted as a. Substituents on the 8, 9, 10, 13, 14, and 17 positions of steroids are projected to Sp, 9a, lop, 13P, 14a, and 17P positions, respectively. p-Sitosterol (or sitosterol) (108) (Fig. 14) is widely distributed in the plant kingdom. a- and P-Ecdysones isolated from silk worm (Bombyx rnori) have steroid skeletons, and are well known as molting hormones. Compounds with similar structure to the ecdysones were isolated from plants (e.g., Podocarpus and Taxus spp.), and are referred to as phytoecdysones [e.g., ponasterone A (109)] (Fig. 14) [79].
C. Tropolones Tropolones are nonbenzenoidaromaticcompoundshaving a seven-memberedenolone structure. They occur in Cupressaceae plants and exhibit antimicrobial activity. Examples
225
Chemistry of Extractives
B i s a b o lFaanren e s a n e
trans-Farnesol 69
(+) -P-Bisabolene 70
(+) -Juvabione
71
Cuparane
Caryophyllane Germacrane
Germacrone (+) -Costunolide 72 73
+-Caryophyllene 74 (-)
(+) -Cuparena
75
Eudesmane
OH
P-Eudesmol 76
(-) -CryptoT-Cadinol meridiol 78 77
FIGURE 11 Examples of sesquiterpenes.
of this class are shown in Fig. 15a. Hinokitiol(P-thujaplicin) (111) was isolated from Charnaecypuris ruiwunmsis by Nozoe [80,81]. a,P, and y-Thujaplicins, (110), (lll),and (112), were isolated from Thuju plicufu by Erdtman [82]. Tropolones are composed of 10 or 15 carbon atoms, and they have been regarded as mevalonate origin, i.e., a subclass of isoprenoids. Recently this has been supported by feedingexperiments.[“C]Mevalonic acid wasfound to beincorporatedinto hinokitiol (111) in suspensioncultures of Cupressus lusitunicu, suggesting that hinokitiol (111) is elaborated via the mevalonate pathway [83].
226
Umezawa
Guaiane
(-)
-Guaiol
79
Aramadendrane
Himachalane
(+) -Aromadendrene
(- 1 -a-Himachalene
80
81
Acorane
Chamigrane
Cedrane
Thuj o p s a n e
q y-Acora-
P-Chamigrene
diene
83
a-Cedrene 84
Thujopsene 85
82
FIGURE 11 Continued
On the other hand, the tropolone structure and aromatic ring of colchicine (114) (Fig. 15b),which is analkaloidfrom Colchicum autumnale, arederivedfromtyrosineand phenylalanine, respectively [84]. Thus colchicine (114) is a phenylpropanoid compound butnot an isoprenoid. In addition,tropolonesoccurring in microorganismsarebiosynthesized via the acetate-malonate pathway [85].
VIII.
QUINONES
Various types of quinones occur in many plant families, and most of them are benzoquinones, naphthoquinones, or anthraquinones. Most of the quinones found in nature are p quinones, but o-quinones also exist [86]. Spica1 examples of this class are shown in Fig. 16. Quinones are biosynthesized via various pathways, i.e., the shikimate, the mevalonate, and the acetate-malonate (polyketide) pathways [2]. Quinones are pigments and have various biological activities. Juglone (116), which occurs in black walnut (Juglans nigra), is skin-irritating [87-891. This compound is also well known as an allelochemical [90]. Tectoquinone (117) and related compounds have strongantitermite activity [91]. Mansonone A (118) and its congenercause allergies [89,92].
227
Chemistry of Extractives
Phytane
LJwwLL OH
m
HO-
OH
Plaunotol87
Phytol 86
Labdane
(+) -transCommunic acid 88
Pimarane,
Isopimarane
(-) -Sandaracopimaric acid
(+) -Pimaric acid 89
90
Nagilactone
Abietane
& p!?
COOH
(-) -Abietic acid
@ H 0
(+) -FerruginolInumaki-Nagilactone 92 lactone A 94
91
A
93
FIGURE 12 Examples of diterpenes.
IX. TANNINS Tannins are water-soluble phenolic compounds having molecular weights between500 and 3000. Besides giving the usual phenolic reactions, they have special properties such as the ability to precipitate alkaloids, gelatin, and other proteins [93,94]. This class of compounds also has high astringency, and gives blue or green coloration with femc chloride. Tanninsare distributed widely in wood, bark, andleaves of many plants. Tannins are classified into hydrolyzable and condensed tannins.
Umezawa
228
ent -Kaurane
ent-Gibberellane
Ginkgolide
COOH (-)
-Kaurene
95
Gibberellin
A19
Ginkgolide B 97
96
Taxane
10-Deacetylbaccatin I11
Taxol 99
98
FIGURE 12 Continued
Hydrolyzable tannins (Fig. 17a) are esters of an aliphatic poly01 and phenolic acids (Fig. 17b), and can be hydrolyzed into the components. As shown in Fig. 17a, galloyl, hexahydroxydiphenoyl, and depside galloyl groups are esterified to the polyol, generally D-glucose. Hydrolyzable tannins that give gallic acid (120) by hydrolysis are referred to as gallotannins, while compounds that afford ellagic acid (122) are referred to as ellagitannins. Hexahydroxydiphenic acid (121) is lactonized to give rise to ellagic acid (122) in the hydrolysis. Some ellagitannins [e.g., casuarinin (119)] have C-glycosidic structures. Two different pathways have been proposed for the biosynthesis of the phenolic unit, gallic acid (120). One is P-oxidation of the side chain of cinnamates to give gallic acid (120), while the other is direct conversion of 3-dehydroshikimate to gallic acid (120) [95]. Recently, it has been shown that formation of gallic acid (120) via cinnamic acids can be ruled out as a major pathway in the fungus Pllycornyce.7 blakesleeanus and in young leaves of Rhus typhirza, and gallic acid (120) is probably formed from an early intermediate of the shikimate pathway, most probably 3-dehydroshikimate [96]. In the pathways to hydrolyzable tannins, the first specific intermediate is P-glucogallin ( l-O-galloyl-P-D-glucose), which is formed from UDP-glucose and gallic acid (120). Then, P-glucogallin is
229
Chemistry of Extractives
Lanostane
Dammarane
Euphane
H3CO"
Abieslactone 100
Limonoid
Dammarenediol I 101
Quassinoid
Euphol 102
Lupane
Oleanane
$$
,8
H0
0
H
OH
Cedrelone 103
Quassin 104 -
P-Amyrin
Betulin ( R S E , O E ) 105
Betulinic
107
acid
(R=COOH) 106
FIGURE 13 Examples of triterpenes.
converted to pentagalloylglucose and gallotannins. Enzymes which catalyze these conversions from gallic acid (120) to gallotannins have been studied intensively by Gross and co-workers, summarized in the review by Gross [97]. Condensedtannins(proanthocyanidins)(Fig.17c)areoligomers and polymersof polyhydroxyflavan-3-01 units [35]. The repeating unit is connected through C4-C6 or C4-C8 bonds. 3-Hydroxyl groups of condensed tannins are often galloylated (e.g., tannins of Diospyros kaki) [98]. Condensation of flavan-3,4-diols and flavan-3-01s may give rise to proanthocyanidins (condensed tannins), but possible mechanisms for the process and their enzymology are still unknown. In spite of their difference in the basic structures, hydrolyzable and condensed tannins have a similarity in that they have many phenolic units and therefore are often called plant polyphenols [94]. Besides the phenolic nature, tannins have the following general characteristics: antioxidant and radical-scavenging activities and the ability to complex with
Umezawa
230
5P-Steroid 5a-Steroid
p-sitosterol
Ponasterone A
108
109
FIGURE 14 Examples of steroids. R: alkyl group.
a-Thujaplicin 110
Einokitiol (P-Thujaplicin)
y-Thu japlicin 112
111
Nootkatin 113
H3coq H&O
H3C0
CH3
.
0 OCH3
Colchicine 114 FIGURE 15 Examples of tropolones.
231
Chemistry of Extractives
OCH3
H3C0
0
0 118
0
J'uglone
2,C-Dimethoxyp-benzoquinone 117 16
TectoquinoneMansonone
A
1
115
FIGURE 16 Examples of quinones.
R=
yo
CO
/OR
OH
RO&&&%' OR Hydrolysable
tannin -
OH OH Hexahydroxydiphenoyl group
Depside galloyl group
OH
l
.n 119
(b)
Gallic acid
120
Haxahydroxydipbenic acid
OH Ellagic acid
122
121
FIGURE 17 (a): Hydrolyzableandcondensedtannins. of (c): hydrolyzable tannins.
(b): phenolic acids whicharecomponents
Umezawa
232
metal ions and with other molecules such as proteins, polysaccharides, and alkaloids [54]. These properties underlie their biological activities as well as their industrial applications. Tannins exhibit various biological and pharmacological activities, e.g., bacteriocidal action, inhibition of HIV replication, as well as astringency [37,54]. Inhibitory effects of condensed tannins on the activities of Streptococcus sobrins glucosyltransferases involved in dental caries formation were also reported [99]. Recently, the role of plant phenolics in diets is attracting considerable interest, since epidemiological investigations suggested that the consumption of beverages containing plant phenolics (such as tannins and flavonoids), in particular, green tea and red wines, reduced the risk of certain degenerative diseases [54,100]. Recent study demonstratedthat the iron-chelating properties of polyphenols contribute to limit the growth of microorganisms [ l o l l . The ability of tannins to complex proteins has long been utilized for tanning agents in leather manufacturing,while that to complexmetal ions hasbeenappliedtodyeing [37,54].Condensed tannins, especiallywattle (ormimosa) tannins, havebeenused to produceadhesives for wood-basedmaterialssuchas particle board and plywood.The tannin adhesives have been successfully commercialized especially in South Africa, Australia, and New Zealand [ 102- 1041. Many reviews of chemical properties, biological significance, and commercial significance of tannins are available in a recent book [105]. Mechanisms of tannin-protein complexation will be described briefly in Section X1.B.
X.
OTHER COMPOUNDS
Besides the compoundsmentionedabove,sugars, triglycerides andwaxes,monomeric aromatic compounds and phenols, alkaloids, etc., occur as extractives in woody plants.
A.
Sugars
D-Glucose and D-fructose are found, along with sucrose, in the sapwood of woody plants, while L-arabinose is found in heartwood [ 1061. Larches (Larix spp.) contain significant amounts (IO-25%) of a water-extractable arabinogalactan [ 1071.
B. Glyceridesand Waxes Glycerides are esters of glycerol and long-chain fatty acids. Among the glycerides, triesters (triglycerides) are dominant. Triglycerides of pine woods cause pitch trouble in ground wood pulping. Waxes are complex mixtures of aliphatic compounds, and a majority of these compounds are wax esters composed of fatty acids and fatty alcohols, hydrocarbons and derivatives, long-chain fatty acids, and long-chain fatty alcohols [ 1081. C.
MonomericAromaticCompounds
Phenylpropanoid monomers are distributed widely in plants, including woody plants. Coniferin (124) and syringin (125) (Fig. 18), aglycons of which are precursors of lignins and lignans, were isolated from many woody plants [109,110]. A soil bacterium, Agrohacteriumtumefaciens, can initiate the neoplastic disease called crown gall on dicotyledonous plants. Tumor-inducing plasmid of the bacterium is used to construct a useful vector to produce transgenic plants. Virulence gene expression
233
Chemistry of Extractives
OH R=E
OH
Coni feryl alcohol 14
R=H Coniferin 124
R=OCH3
Sinapyl alcohol 123
Anethole 126
R=OCE3
Syringin 125
Eugenol 127
Umbelliferone 130
Safrole 128
Cinnamaldehyde 129
Aesculetin 131
R Urushiol 132 R=ClSH25-31 FIGURE 18 Examples of monomeric aromatic compounds.
of the bacterium is activated by coniferyl alcohol (14) and sinapyl alcohol (123) [ l I l ] (Fig. 18) as well as acetosyringone (3’,5’-dimethoxy-4’-hydroxyacetophenone) [ 1 121. Various phenylpropanoid monomers are components of essential oils, for example (Fig. 18), anethole (126) (star aniseed oil), eugenol (127) (clove oil), safrole (128) (sassafras oil), and cinnamaldehyde (129) (cassia oil), which have been used for spice and perfume. Coumarins constitute another class of phenylpropanoids which have 2H- 1 -benzopyran-2-one structure. They are distributed widely in plants, particularly Umbelliferae and Rutaceae [ 113- 1 151. Two examples, umbelliferone (130) and aesculetin (131), are shown in Fig. 18. Biological activities of coumarins are reviewed in the literature [37]. Urushiol (132) (Fig. 18) is a major component of urushi (Japanese lacquer), milky exudate from urushi (Rhus vernicijlua), which has been used to produce japan (Japanese lacquer ware) [ 116,1171.
234
Urnezawa
0 "+,/
OCH3
N
H
/
Berberine 133
H% H3COys
Quinine 134
9 H '
HH0
0 OH
-tine
,I
OCH3 OCH3
135
H 3 c 0H 3 ~ C: O H" w
0 OCH3
Yohimbine Strychnine Reserpine
OCH3 OCH3
136
Camptothecin FIGURE 19 Examples of alkaloids.
D. Alkaloids Although the occurrence of alkaloids is much less than other wood extractives, most of them are of considerable interest due to their biological activity. Examples of alkaloids from woody plants are as follows [37,118- 1201 (Fig. 19): berberine (133) from Phellodendron arnurense, which is antibacterial; quinine (134) from Cinchona pubescens, which is employed for the treatment of malaria; emetine (135) from Cephaelisipecacuanha, which is anamebicide;yohimbine (136) from Pausinystalia yohimbe, which is a selective inhibitor of the presynaptic a-2-adrenergic receptors; strychnine (137) from S t r y c h n o s n u - v o m i c a , a very toxic alkaloid; reserpine (138) from Rauwolfia serpentina, which is antihypertensive; and camptothecin (139) from Camprotheca acurninata. which is antitumor.
XI.
CONTRIBUTION OF EXTRACTIVES TO THE PROPERTIES OF WOOD AND UTILIZATIONOF WOOD EXTRACTIVES
Extractives of wood influence various properties of wood, e.g., color, fragrance, and durability. Some extractives have injurious effects on human health[89]. Troubles in pulping processes and adhesion in production of wood-based materials are sometimes due to extractives. They are described in detail in a book [ 1211 and outlined byKaiin the first edition of this book [122]. Therefore, several topics in these fields are described briefly in this section.
Chemistry of Extractives
A.
235
AcousticProperties
Recently, acoustic properties and internal friction (loss tangent, tan S) of several woods and a cane have been observed to be strongly influenced by extractives. The term tan S is an indication of decrement of vibration of solid materials, and materials with lower tan S exhibit higher sound radiation. Methanol extraction of heartwood specimens of western red cedar (Thuja plicata), which is usedfor the top plate of the guitar, increased tan S values by 15.3-36.9% [ 123,1241. The same effect of methanol extraction was observed for rosewood (Dalbergia spp.), black cherry(Prunus serorina), and padauk (Pterocarpus indicus),whereas no effects of heartwood contents or methanol extractives were detected in bubinga (Guibourtia demeusei) [ 123,1241. Pernambuco (Guilandinaechinata syn. Caesalpiniaechinata) andcane (Arundo donax) have been used for violin bows and reeds of woodwind instruments, respectively. Water extracts from pernambuco reduced tan S value [ 1251, while in the case of air-dried cane, water extracts increased tan S value [126]. It was suggested that the water extracts of the cane consisted mainly of oligoglucans [126].
B. Tannin-ProteinComplexation The ability to complex with proteins is one of the most important features of tannins, and the mechanisms for tannin-protein complexation have long been studied. These studies clarified effects of environmental factors (such as pH, temperature, and ionic strength) on the process, and the following three principal features of tannin structure and properties which are important in the complexation with protein have been established: molecular size, conformational flexibility, and water solubility of the tannin. [54,94,127-1291. The precipitation ability increases with an increase of the degree of polymerization of condensed tannin [130], while in the case of hydrolyzable tannin this ability is enhanced with the addition of galloyl ester group [ 13 l]. Selective interaction of the condensed tannin from Sorghum bicolor with various proteins was also investigated, and it was reported that proline-rich and flexible proteins have high affinity for the polyphenol [ 1321. As for the mode of interaction between tannins and proteins, involvement of hydrogen bonding and hydrophobic interaction was suggested [ 1271. Although the relative importance of these two types of interactions remains uncertain, the initial association of protein-polyphenol by hydrophobic interaction followed by reinforcement of the association by hydrogen bonding was proposed [ 1271. Since tannins have complicated structures, synthetic tannin models which have definite structures are useful to elucidate mechanisms of tannin-protein complexation. Based onexperimentswithaseries of synthesizedcondensedtanninmodels, the distribution pattern of the phenolic hydroxyl group in the tannin molecule, but not the existence of odihydroxyphenyl groups, was found to be important for higher protein-precipitating capacity [ 133,1341. Two mechanisms were proposed for tannin-protein co-precipitation [94,127]. One is a “cross-linking mechanism,” in which one tannin molecule binds more than two protein molecules simultaneously to form an aggregate to be precipitated. The other is a “twostage precipitation mechanism,” which consistsof initial complexation of tannin molecules to a protein molecule to form a complex, followed by aggregation of the complexes to give precipitates. Recently, a series of hydrolyzable tannin models has been synthesized, and studies withthe models suggested that the two-stage mechanism is involved in tanninprotein co-precipitation [129,135,136].
Umezawa
236
C. Antitumor Taxol and Podophyllotoxin Recently, phytochemical studies of yew trees (Taxus spp.) have been developed exponentially [ 1371. This is due mainly to the plants’ producing taxane diterpene, taxol (99), which has strong antitumor activity. Taxol (99) is one of the most promising anticancer drugs and has been marketed under the name of TaxoP. Paclitaxel is the generic name for TaxoP. Because of great familiarity with the word taxol, however, it is used in this review in lieu of paclitaxel. Taxol (99) is present only in trace amounts in Taxus spp. (e.g., 0.0001-0.069% from 7: brevifolia bark) [ 1381. The sources of taxol (99) and related taxaneswerereviewed [ 1391. Interestingly, Taxomyces andreanae,an endophytic fungus of 7: brevifolia, produces taxol (99) andbaccatin 111 whenincubated in a semisynthetic liquid medium,although the quantities detected are very low (24-50 ng of taxolk) [140]. The limited production of taxol (99) in nature as well as the projected needs for the compound and its unique chemical structure have provided a very challenging target for syntheticorganicchemists.Recently,two total syntheses of this compoundhavebeen reported independently [ 141-1431. The production of taxol (99) through semisynthesis fromthemore readily available 10-deacetylbaccatin 111 (98) is nowwellestablished [ 144,1451. The biosynthesis of taxol (99) and its production by cultured cells have also received much interest. Recently,taxadienesynthasecatalyzing the cyclization of the universal diterpene precursor, geranylgeranylpyrophosphate (60), to the taxanesystem [taxa4(5), 1 l( 12)-diene] in a single enzymatic step was purified and characterized [ 1461. Very recently, Eisenreich et al. showed that the taxane ring system is not biosynthesized via mevalonate [73]. Production of taxol (99) by cultured cells is reviewed in the literature [120,145,147]. An aryltetralin lignan podophyllotoxin (7)has strong antitumor and antimitotic activity [4,5,20,148]. Since the lignan possesses severe gastrointestinal toxicity, semisynthetic derivatives of podophyllotoxin (7)have been developed to avoid the toxicity. Etoposide, which isone of the derivatives,hasbeenusedsuccessfully for cancerchemotherapy [5,148]. Podophyllotoxin (7)and its congeners occur in root and rhizome of Podophyllum spp. as well as other plants including woody plants, e.g., callus culture of Callitris drummondii (Cupressaceae) and leaves of Juniperus spp. (Cupressaceae) [20,148]. These lignans are elaborated from matairesinol [5,9,149,150].
D.
Pitch Trouble in Pulp and Paper Making
Wood extractiveshavecaused technical andeconomic pitch problems in the pulpand paper industry. Recently,twotypes of biochemicaltreatmentshavebeendeveloped to alleviate the problems. One employs enzymes, and the other uses a microorganism. Japanese red pine (Pinus densijora) isan important raw material for groundwood pulp. The wood contains significant amounts of resinousmaterialswhichcause pitch trouble in groundwood pulp process. The trouble can be partly avoided by seasoning the logs. Recently, lipase-catalyzed hydrolysis was foundto reduce triglycerides in the resinous materials to 70%, when the enzyme was added to groundwood pulp at 9000 U/kg. This treatment reduced the pitch deposits remarkably, and allowed the use of unseasoned logs up to 50% of total wood supply without pitch troubles [ 15 1,1521. Theother is a biological approach to decreasingextractivesfrom wood prior to pulping using the fungus Ophiostoma piliferum. A 2-week treatment of pine chips (50%
Chemistry of Extractives
237
Pinus taedcl and 50% Pinus virginiuna) with the fungus reduced ether-extractable pitch components by 22% compared with chips seasoned naturally for 2 weeks. GC-MS analysis of pitch components in fresh chips and in fungus-treated chips showed significant declines in the concentrations of triglycerides, fatty acids, and resin acids [ 1531.
REFERENCES 1. N. Migita, Y. Yonezawa, and T. Kondo (eds.), Wood Chemistry (in Japanese), Kyoritsu Shuppan, Tokyo ( 1 968). 2. T. Higuchi, Biochemistry and Molecular Biology of Wood, Springer-Verlag, Berlin (1997). 3. C. B. S. Rao (ed.), Chemistry of lignans, AndhraUniversityPress,AndhraPradesh,India ( 1978). 4. W. D. MacRaeandG.
5.
6. 7. 8. 9. IO. 1I.
H. N.Towers, Phytochemistry,23: 1207 (1984). D. C. Ayres and J. D. Loike. Lignans:Chemical,BiologicalandClinicalProperties, Cambridge University Press, Cambridge, U.K. (1990). R.D.Haworth, Ann. Rep. frog. Chem., 33: 266 (1936). 0. R.Gottlieb, Phytochernistry, 11, IS37 (1972). 0. R. Gottlieb, Fortscht:Chem. Org. Nuturst., 35, 1 (1978). T. Umezawa, in Biochetnistr?:andMolecularBiology of Wood, (T. Higuchi, ed.), SpringerVerlag, Berlin, pp. 181 - 194 ( 1997). 0. R. Gottlieb, in Chemistry of lignuns (C. B. S. Rao, ed.), Andhra University Press, Andhra Pradesh, India, pp. 277-305 ( I 978). T. Umezawa,L. B. Davin,and N. G.Lewis, Biochem.Biophys.Res.Cotnmun.. 171: 1008
(1990). 12. A. Chu, A. Dinkova, L. B. Davin, D. L. Bedgar, and N. G. Lewis, J . B i d . Chern., 268: 27026 ( 1993). 13. P. W. Park,H.-B.Wang,L. B. Davin, and N. G. Lewis, Tetrahedron Lett., 35: 4731 (1994). 14. A. T. Dinkova-Kostova, D. R. Gang, L.B. Davin, D. L.Bedgar, A. Chu, and N. G. Lewis, J. B i d . Chern., 271: 29473 (1996). IS.
16. 17. 18. 19. 20. 21. 22. 23. 24. 25.
26. 27. 28. 29. 30. 3I .
L. B. Davin, H.-B. Wang, A. L. Crowell, D. L.Bedgar, D. M. Martin, S. Sarkanen, and N. G. Lewis, Sciencc~,275: 362 (1997). T. Umezawa and M. Shimada, Biosci.Biotechnol.Biochem.. 60: 736 (1996). S. Suzuki, T. Umezawa,andM.Shimada, Biosci.Biofechnol.Biochem., 62: 1468(1998). J . D. Orr and D. G. Lynn, Plant Physiol., 98: 343 (1 992). T. Katayama and Y. Kado, J . Wood Sci., 44: 244 ( 1998). T. Umezawa, MokuzaiCakkaishi. 42: 91 1 (1996). L. U. Thompson, M. M. Seidl, S. E. Rickard, L. J. Orcheson, and H. H. S. Fong, Nutrition and Cancer, 26: 159 ( I 996). T. Y. Shen, S.-B. Hwang, M. N. Chang, T. W. Doebber, M.-H. T. Lam, M. S. Wu, X. Wang, G. Q. Han, and R. Z . Li, Proc. N r d . Acad. Sci. USA, 82: 672 (1985). A. M.Clark, F. S. El-Feraly, and W.-S. Li, J . Pharmaceut. Sci., 70: 951 (1981). K. Watanabe,H.Watanabe, Y. Goto, M. Yamaguchi, N. Yamamoto, and K. Hagino, Plantu Med., 49: 103 (1983). D. A. Whiting, Naturcrl Prod.Rep., 4 : 499(1987). D. A.Whiting, NaturalProd. Rep., 7 349(1990). R. S. Ward, Nuturd Prod. Rep., 12: 183 (1995). T. Nikaido, T. Ohmoto, H. Noguchi, T. Kinoshita, H. Saitoh, and U. Sankawa, Plantcl Med., 43: 18 (1981). J. Kinjo, J. Furusawa,and T. Nohara, Tetrahedron L e f t . , 26: 6101 (1985). A. J . Birch and A. J. Liepa, in Chemistr~y ofLignans (C. B. S. Rao, ed.), Andhra University Press, Andhra Pradesh, India, pp. 307-327 (1978). Y. Kai, H. Kuroda, and F. Teratani, Mokuzai Gakkaishi. 18: 3 1 S ( I 972).
238
Umezawa
32. K. Takahashi, Mokuzai Gakkaishi, 2 7 654 (198 l ) . 33. H. Ohashi, H. Hayashi, M. Yamada, and M. Yasue, Res. Bull. Fac. Agr. Gifu. Univ., 52: 131 (1987). 34. H. Funakoshi, K. Nobashi, and T. Yokota, Mokuzai Gakkaishi, 24: 141 (1978). 35. L. J. Porter, in Methods in Plant Biochemistry, Vol. l . Plant Phenolics (J. B. Harborne, ed.), Academic Press, London, pp. 389-419 (1989). 36. J. B. Harborne, in Natural Products of Woody Plants I, (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 533-570, (1989). 37. J. Bruneton, Pharmacognosy, Phytochemistry, Medicinal Plants (C. K. Hatton, transl.), Lavoisier, Paris (1995). 38. J. B. Harborne (ed.), The Flavonoids: Advances in Research Since 1986, Chapman & Hall, London (1994). 39. J. B. Harborne, T. J. Mabry, and H. Mabry (eds.), The Flavonoids, Chapman & Hall, London (1 975). 40. J. B. Harborne and T. J. Mabry (eds.), The Flavonoids: Advances in Research, Chapman & Hall, London (1982). 41. J. B. Harborne (ed.), The Flavonoids: Advances in Research Since 1980, Chapman & Hail, London (1988). 42. W. HellerandG.Forkmann,in The Flavonoids: Advances in Research Since 1986 (J. B. Harborne, ed.), Chapman & Hall, London, pp. 499-535 (1994). 43. K.HahlbrockandH.Grisebach,in The Flavonoids (J. B.Harborne, T. J. Mabry,andH. Mabry, eds.), Chapman & Hall, London, pp. 866-915 (1975). 44. R. K. Ibrahim and L. Varin, in Methods in Plant Biochemistry, Vol. 9, Enzymes of Secondary Metabolism (P. J. Lea, ed.), Academic Press, London, pp. 99- 131 ( 1 993). Plant Mol.Biol., 24: 743 45. F. Sparvoli,C.Martin,A.Scienza,G.Gavazzi,andC.Tonelli, (1994). 46. G. Forkmann, in Polyphenolic Phenomena (A. Scalbert, ed.), INRA, Paris, pp. 65-71 (1993). 47. G. Forkmann, in The Flavonoids: Advances in Research Since 1986 (J. B. Harborne, ed.), Chapman & Hall, London, pp. 537-564 (1994). 48. B.W. Shirley, W. L. Kubasek, G. Storz, E. Bruggemann, M. Koornneef, F. M. Ausubel, and H. M. Goodman, The Plant l.,8: 659 (1995). Recent Advances in 49. R. A. Dixon, C, A. Maxwell, W. Ni, A. Oommen, and N. L. Paiva, in Phytochemistry,Vol. 28, Genetic Engineering of PlantSecondary Metabolism (B. E. Ellis, G. W. Kuroki, and H. A. Stafford, eds.), Plenum Press, New York, pp. 153-178 (1994). 50. C. A. Williams and J. B. Harborne, in Methods in Plant Biochemistry, Vol. I , Plant Phenolics (J. B. Harborne, ed.), Academic Press, London, pp. 421-449 (1989). 51. P.M. Dewick, in The Flavonoids: Advances in Research (J. B. Harborne and T. J. Mabry, eds.), Chapman & Hall, London, pp. 535-640 (1982). 52. K. Hayashi, Plant Pigments, an Introduction to Research and Experiments (enlarged ed.) (in Japanese), Yokendo, Tokyo (1988). 53. T. Goto and T. Kondo, Angew. Chem. Int. Ed. Engl., 30: 17 (1991). 54. E. Haslam, J. Natural Prod., 59: 205 (1996). 55. E. Middleton, Jr., and C. Kandaswami, in The Flavonoids: Advances in Research Since 1986 (J. B. Harborne, ed.), Chapman & Hall, London, pp. 619-652 (1994). 56. T. Okuda, in Polyphenolic Phenomena (A. Scalbert, ed.), INRA, Paris, pp. 221-235 (1993). 57. T,P. Jungblut, J.-P. Schnitzler, W. Heller, N. Hertkorn, J. W. Metzger, W. Szymczak, and H. Sandermann, Jr., Angew. Chem. Int. Ed. Engl., 34: 312 (1995). H. Ziegler, Trees, 5 : 203 (1991). 58. E. A. Magel, A. Drouet, A. C. Claudot, and 59. E. Magel and B. Hubner, Bot. Acta, 110: 314 (1997). 60. T. Norin, in Natural Products of Woody Plants I (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 512-533 (1989). 61. H. Kindl, in Biosynthesis and Biodegradation of Wood Components (T. Higuchi, ed.), Academic Press, Orlando, FL, pp. 349-377 (1985).
Chemistry of Extractives
239
62. H. Kindl, Hoppe-Seylerh Z. Physiol. Chem., 352: 767 (1971). 63. R. Gehlert, A. Schoppner, and H. Kindl, Mol. Plant-Microbe Interact., 3: 444 (1990). 64. R. Hain, H.-J. Reif, E. Krause, R. Langebartels, H. Kindl, B. Vornam, W. Wiese, E. Schmelzer, P. H. Schreier, R. H. Stocker, and K. Stenzel, Nature, 361: 153 (1993). 65. H. Erdtman, Tappi, 32: 346 (1949). 66. P. Cleason, P. Tuchinda, and V. Reutrakul, J . Indian Chem. Soc., 71: 509 (1994). 67. G . M. Keserii and M. N6grBdi, in Studies in Natural Products Chemistry. Vol. 17 (Atta-urRahman, ed.), Elsevier, Amsterdam, pp. 357-394 (1995). 68. P. J. Roughley and D. A. Whiting, Tetrahedron Lett., 1971: 3741. 69. T. Inoue, N. Kenmochi, N. Furukawa, and M. Fujita, Phytochemistry, 26: 1409 (1987). 70. N. Watanabe, Y. Uraki, and Y. Sano, “Biosynthesis of Diarylheptanoids in Betulaceae”, in 71. 72. 73. 74. 75. 76.
Abstracts of the 40th Anniversary Conference of the Japan Wood Research Society, Tokyo, Japan, p. 420 ( 1 995). M. Rohrner, M. Knani, P. Simonin, B. Sutter, and H. Sahm, Biochem. J., 295: 517 (1993). M. Rohmer, M. Seemann, S. Horbach, S. Bringer-Meyer, and H. Sahm, J. Am. Chem. Soc., 118: 2564 (1996). W. Eisenreich, B. Menhard, P. J. Hylands, M. H. Zenk, and A. Bacher, Proc. Natl. Acad. Sci. USA, 93: 643 1 ( 1996). S. Dev, in Natural Products of Woody Plants I1 (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 691-807 (1989). W. R. Nes, in Natural Products of Woody Plants I1 (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 808-842 ( 1 989). J. D. Connolly and R. A. Hill, Dictionary of Terpenoids, Vols. 1-3, Chapman & Hall, London
(1991). 77. R. Croteau and M. A. Johnson, in Biosynthesis and Biodegradation of Wood Components (T. Higuchi, ed.), Academic Press, Orlando, FL, pp. 379-439 (1985). 78. S. Kobayashi, C . Ishibashi,A.Morita, H. Masuda,andA.Ogiso, Pharmacometrics (Oyo kkuri), 24: 599 (1982). 79. K. Nakanishi, M. Koreeda, S. Sakai, M. L. Chang, and H. Y. Hsu, Chem. Commun., 1966: 915. 80. T. Nozoe, Bull. Chem. Soc. Jap., 11: 295 ( 1936). 81. T. Nozoe, Fortschr Chem. Org. Nuturst., 13: 232 (1956). 82. H. Erdtman, Progr. Org. Chem.. 1: 22 (1952). 83. K. Sakai, T. Yamaguchi, and R. Itose. Mokuzai Gukkaishi, 43: 696 (1997). 84. A. R.Battersby, T. A. Dobson, D. M. Foulkes, and R. B. Herbert, J. Chem. Soc. Perkin 1, 1730 (1972). 85. M. C. O’Sullivan and J. M. Schwab, Bioorg. Chem., 23: 131 (1995). 86. A. J.J. van den Berg andR. P. Labadie, in Methods in P h l t Biocherni,ytl;y, Vol. I (J. B. Harborne. ed.), Academic Press, London, pp. 451-491 (1989). 87. E. P. Swan, in Nrrtural Products sf Woody P1unt.s I1 (J. W. Rowe, ed.). Springer-Verlag, Berlin, pp. 931-952 ( 1989). 88. J. W. Rowe and A. H. Conner. Generul Tech. Rep. Forest Pmd. h b . Mudison, 18: 22 ( 1 979). 89. B. Hausen. Woods Injurious to Humun Health: A M a n ~ ~ ndel , Gruyter, Berlin ( 1981). 90. E. L. Rice, Allelopcrthy. 2nd ed.. Academic Press. Orlando, FL (1984). 91. W. Sandermann and M. H. Simatupang, Hol: u l s Roh- und Werkstoflff; 24: 190 (1966). 92. N. Tanaka. M. Yasue, and H . Imamura. Tetrahedron Lett.. 1966: 2767. 93. T. Swain and E. C. Bate-Smith, in Cortlparative Biochemistry, Vol. 3 (M. Florkin and H. S. Mason, eds.). Academic Press, New York, pp. 755-809 (1962). 94 E. Haslam, Plnnt Po1yphenol.s. Cambridge University Press, Cambridge, U.K. (1989). 95. E.Haslamand Y. Cai. Nuturd Prod. Rep., 11: 41 ( 1994). 96. I. Werner, A. Bacher, and W. Eisenreich. J. Riol. Chem., 272: 25474 (1997). 97. G . G. Gross. in Methods i n Plunt Bioc.k~.rlri.str?: W . 9, Enzymes of Seconrltrt:\. Metcrl~olisrn (P. J. Lea, ed.). Acadcmic Press, London. pp. 25-43 (1993).
240
Umezawa
98. T. Matsuo and S. Ito, Agric. Biol. Chem., 42: 1637 (1978). 99. T. Mitsunaga, I. Abe, M. Kontani, H. Ono, and T. Tanaka, J. Wood Chem. Technol., 1 7 327 ( 1997). 100. A. L. Waterhouse, Chem. Ind.. 1995: 338. 101. I. Mila, A. Scalbert, and D. Expert, Phytochemistry, 42: 155 1 (1996). 102. A. Pizzi, in Polyphenolic Phenomena (A. Scarbert, ed.), INRA, Paris, pp. 267-274 (1993). 103. Y. Yazaki, Proc. 18th Symp. on WoodAdhesion, Tokyo,pp. 36-48 (1997). 104. H. L. Hergert, in AdhesivesfromRenewableResources,ACS Synzp. Ser: 385 (R. W. Hemingway and A. H. Conner, eds.), American Chemical Society, Washington, DC, pp. 155-171 (1989). 105. R. W. Hemingway and P. E. Laks (eds.), Plant Po/yphenols, Plenum Press, New York (1992). 106. J. N.BeMiller,in NaturalProducts of WoodyPlants I , (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 155-1 78 (1989). 107. T. E. Timell, Wood Sci. Technol., I : 45(1967). 108. P. E. Kolattukudy and K. E. Espelie, in NaturalProducts of WoodyPlants I (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 304-367 (1989). 109. M. Terazawa, H. Okuyama, and M. Miyake, Mokuzui Gakkuishi, 30: 322 (1984). 110. M. Terazawa and M, Miyake, Mokuzai Gakkaishi, 30: 329 (1984). 1 1 1. P. A. Spencer and G. H. N. Towers, Phytochemistry, 2 7 2781 (1988). 112. S. E. Stachel, E. Messens, M. van Montagu, and P. Zambryski, Nature, 318: 624 (1985). 113. R. D. H.Murray, Forrschr: Chem.Org.Nuturst., 35: 199 (1978). 114. R. D. H. Murray, Nuturul Prod.Rep., 12: 477, (1995). 115.
116. 117. 1 1 8.
119. 120. 12 I . 122. 123. 124. 125. 126. 127. 128. 129. 130. 13 I .
132. 133.
134. 135. 136. 137. 138.
0. Theander and L. N. Lundgren, in Natural Products of Woody Plunts I (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 369-399 (1989). W. E. Hillis, in NaturalProducts o f WoodyPlants I (J. W. Rowe,ed.), Springer-Verlag, Berlin, pp. I - 13 ( 1989). W. E. Hillis, Heartrt'ood and Tree Exudates, Springer-Verlag.Berlin, pp. 59-60 (1987). C. W. W. Beecher, N. R. Farnsworth, and C. Gyllenhaal, in Nuturul Products of Woody Plants II (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 1059-1 164 (1989). S. I. Sakai, N. Aimi, E. Yamanaka, and K. Yamaguchi, in Natural Products of Woody Plunts I (J. W. Rowe, ed.), Springer-Verlag, Berlin, pp. 200-257 (1989). S. Tachibana, Mokuzai Gakkaishi, 41: 967(1995). J. W. Rowe (ed.), Natrtrd Products of Woody Plants. I and 11, Springer-Verlag, Berlin (1989). Y. Kai, in Wood andCellulosicChemistry (D.N.-S. Hon and N. Shiraishi,eds.),Marcel Dekker, New York, pp. 2 15-255 ( 199I ). H. Yano, Holiforsch.,48: 491 (1994). H. Yano, H. Kajita and K. Minato, J . Acous?. Soc. Am., Y6: 3380 (1994). M. Matsunaga, M. Sugiyama, K. Minato, and M. Norimoto, Holiforsch., "TO: 51 1 (1996). E. Obataya, T. Umezawa, F. Nakatsubo, and M. Norimoto. Holz,forsch., 53: 63 (1990). C. M. Spencer, Y. Cai, R. Martin, S. H. Gaffney, P. N. Goulding, D. Magnolato, T. H. Lilley, and E. Haslam, Phytochemistry, 27: 2397 (1988). G. Luck. H. Liao, N. J . Murray, H. R. Grimmer, E. E. Warminski, M. P. Williamson, T. H. Lilley, and E. Haslam, Phytochemistry, 37: 357 ( 1994). H. Kawamotoand F. Nakatsubo, Recent Res. Devel. Phytochem., I : 515(1997). E. C.Bate-Smith, Phytochemistry, 12: 907(1973). E. Haslam, Biochem. J.. 139: 285 (1974). A. E. Hagerman and L. G. Butler, J. B i d . Chenl., 256: 4494(1981). H. Kawamoto, F. Nakatsubo,and K. Murakami, J. Wood Chenz. Technol.. 1 0 59 (1990). H. Kawamoto, F. Nakatsubo,andK.Murakami, J. Wood Chem. Technol.. l o : 401 (1990). H. Kawamoto, F. Nakatsubo, and K. Murakami. Ph?,toc/lerni.stt:v,40: 1503 ( 1995). H. Kawamoto, F. Nakatsubo,and K. Murakami, Phytochemistry, 41: 1427 (1996). G.Appendino, Nrtturul Prod.Rep.,12: 349 (1995). N. Vidensek, P. Lim, A. Campbell, and c. Carlson, J . Nuturul Prod., 53: 1609 (1990).
Chemistry of Extractives
241
139. D. G. I. Kingston, Phcrrnlctcol. Tl~er:.52: 1 (1991). 140. A. Stierle, G. Strobel, and D. Stierle, Science. 260: 214 (1993). 141. R. A. Holton, C. Somoza. H,-B. Kim, F. Liang, R. J. Biediger, P. D. Boatman, M. Shindo, 142. 143. 144. 145. 146. 147. 148. 149. 150.
151.
152. 1 53.
C.C.Smith, S. Kim. H. Nadizadeh, Y. Suzuki,C. Tao, P. Vu, S. Tang, P. Zhang, K. K. Murthi, L. N. Gentile, and J. H. Liu, J. Am. Chem. Soc., 116: 1597 (1994). R. A. Holton, H.-B. Kim, C. Somoza, F. Liang, R. J. Biediger, P. D. Boatman, M. Shindo, C.C.Smith, S. Kim. H. Nadizadeh, Y. Suzuki,C. Tao, P. Vu, S. Tang, P. Zhang, K. K. Murthi, L. N. Gentile, and J. H. Liu. J. Am. Chern. Soc., 116: 1599 (1994). K. C. Nicolaou, Z. Yang, J . J. Liu, H. Ueno, P. G. Nantermet, R. K. Guy, C. F. Claiborne, J. Renaud, E. A. Couladouros, K. Paulvannan, and E. J. Sorensen, Nrrture, 367: 630 (1994). D. G . I . Kingston, in filxurw AnticwlcerAgents:Basic Science crnd CurrentStatus,ACS Syrnp. Ser: 583 (G. I. Georg. T. T. Chen, I. Ojima, and D. M. Vyas, eds.), American Chemical Society, Washington, DC, pp. 203-216 ( 1995). M. Suffness, in fir\-nr~eArzticcrrlcer Agents: Basic Science crud CurrentStatus,ACS Syrnp. Ser: S83 (G. I. Gcorg, T. T. Chen, 1. Ojima,and D.M. Vyas, eds.),AmericanChemical Society, Washington, DC, pp. 1-17 (1995). M. Hezari, N. G. Lewis, and R. Croteau, Arch. Biochem. Biophys., 322: 437 (1995). S. Furusaki, M. Seki, and M. Nakajima, Biosci. Ir~d.,52: 896 (1994). D. L. Sackett, Phtrrmrcol. Tlzer., 59: 163 (1993). P. M. Dewick, in Studies i n Naturol Products Chenlistry, Vol. S. Structure Elucidutiorl (Pcrrt B) (Atta-ur-Rahman, ed.), Elsevier, Amsterdam, pp. 459-503 ( 1 989). A. J. Broomhead. M. M. A. Rahman, P. M. Dewick. D. E. Jackson. and J. A. Lucas. P h y tocherrlistry, 30: I489 ( I99 I ). Y. Fujita, H. Awaji, M. Matsukura, and K. Hata, J q m z Tappi J . , 4.5: 905 (1991). Y.Fujita, H. Awaji, H. Taneda, M . Matsukura, K. Hata, H. Shimoto, M. Sharp, H. Sakaguchi, and K. Gibson, firppi J.. 74: 117 (1992). T. S. Brush, R. L. Farrell, and C. Ho. R ~ p p J., i 77: 155 (1994).
This Page Intentionally Left Blank
7
Chemistry of Bark Kokki Sakai Kyushu University, Fukuoka, Japan
1.
INTRODUCTION
Tree bark usually refers to all tissues external to and surrounding the vascular cambium. It occupies a much smaller volume than the wood of a mature tree stem because fewer bark cellsare produced than wood cells and also because the outermost bark cellsare continuously discarded in most tree species, while wood cells are retained and thus accumulate as the tree grows. In spite of its small volume, the bark plays important roles in a living tree. Tree barks often have developed complex anatomy and/or chemical compositions in order to manifest or maintain three main functions: (1) nutrient transport from the leaves to the rest of the tree, (2) protecting the sensitiveinnercambiumfromdesiccation,and (3) shielding from the environment as the primary defense of the tree against wildfire, mechanicalinjuriescaused by heavy wind, and attacks by phytopathogens,phytophagous insects, larger animals, and so on. The objective of this chapter is to provide the new information about the chemical composition and utilization of tree barks, mainly since 1986. The basic knowledge of bark chemistry and important findings in this field up until 1985 were well stated by Laks in the first edition of this book [ 11.
II. THE FORMATION AND ANATOMY OF TREE BARKS The formation and anatomy of bark are described very briefly, as quite detailed discussions of them were presented by Laks [ l ] . The epidermis. the cortex, and the primary phloem are produced during longitudinal growth from the apical meristem located at the apices of growing roots and branches. The secondary phloem and periderm are formed during radial growth of the tree. Accordingly, the primary phloem remains in only the outermost region of the bark of young trees. In most tree species the outer bark cracks and peels off as the tree grows, due to the successive formation of periderms within the bark and growth of the xylem. Thus the mature bark consists mainly of secondary phloem and periderm, a group of tissues including the phellogen or cork cambium, the phelloderm, and the phellem or cork tissue. As the sec243
Sakai
244
ondary phloem thickness, new periderm is formed within the phloem and any cells to the exterior of the periderm soon die. Most tree barks, therefore, have two zones, the inner bark that contains some living cells and the outer bark or rhytidome that does not contain any living cells. These regions are sometimes compared to the sapwood and heartwood in the xylem, respectively. Recently, Trockenbrodt [2] surveyed and discussed the terminology used in bark anatomy, andsuggestedterms for the tissue zones as illustrated in Fig. 1 . In the barkchemistry field, however, the terms “outer bark” and “inner bark” have been used for “rhytidome” and “secondary phloem up to the last-formed living secondary phloem,” respectively.
111.
CHEMICAL COMPOSITIONAND NONEXTRACTABLE COMPONENTS OF TREE BARKS
As described above, bark consists of the inner bark and outer bark zones. It is therefore preferable to determine the chemical composition accuratelyfor these two zones separately. However, chemical analyses have often been made with the whole bark because separation between the zones is sometimes cumbersome and time consuming, and because for most applications the whole bark is to be utilized. It has been known that chemical analyses by standard methods for wood often give erroneous results due to the presence and variability of suberin and high-molecular-weight tannins which are rarely or never found in wood. Surprisingly, some erroneous data were published evenin 1991 [ 3 ] .Preliminary extractions or corrections for these substances are very important for the accurate analysis of the bark of trees. Some of the general and comprehensive reviews onthe chemical composition of tree barks were referred to by Laks [ l ] . More recent examples of bark analysis are listed in Table 1 to show how different the chemical compositions of the tree bark are from those of wood. In general, bark contains much more extractives, slightly less lignin, and smaller amounts of holocellulose as compared to wood of the same tree. Nonextractable components in the bark consist of polysaccharides (cellulose, hemicellulose,and pectic substances),phenolicpolymers (lignin andhigh-molecular-weight tannins), and cross-linked polyesters (suberin and cutin). Significant parts of hemicellulose
/-
rhytidomc
secondary phlocm u p to thc last fonncd pc’idclnd living sccondaryphlocm calnbiunl xylcm FIGURE 1 Suggested tcrms for the tissue zones resulting from rhytidomc formation. Rcproduccd with permission of IAWA.
Chemistry of Bark
245
TABLE 1 Some BarkAnalyticalResults
(9%of DryMaterials)
Components Species
Extract. Lignin Ash
Holocellul. Cellulose Pentosan
1 % NaOH soh. Ref.
Eucalyptus glohulrts" 0.3
B kh
5 18.6 7.9 2.0
Wd' Populus Hybrid
1
NE388d B kh Wd' Pinus pirznster
28.7
B kh19.1 I? radiata Bkh Wd' I? sylvestris
Bkh Wd' Snlix roridrr
Bkh S. rkinuycrnngi Bkh
8.0
22.3
41.8 5.6
14.1 16.7
43.2 50. I 42.9 84.5
19.6 20.5
30.6 22.5
23.2 44.0 22.7
0.5 "2q.f -26 27.2 1.8
31.4
12.6 8.2
25.7 14.8
59.3 12.5
I1.1F
7.4
54.2"
10.4F
7.9
53.5"
"Twelve-year-old trees. hBark. 'Wood. "Four-year-old trees. 'Estimated by the solid-state "C-NMR method. 'Tannin. 'Alcohol-benzene extract. hAfter extraction with alcohol-benzene
and pectins can be removed during the extraction of tannins with alkaline solutions. This solubility also causes the difficulty in accurate analyses of the bark components. Recent studies on nonextractables in the bark are very limited. A lipidic biopolymer, suberin, is the most important structural component of the cork cell walls, which play the physiologically important role of thermal and hydric insulation in bark tissues. Suberin composition of Cedr-us libani bark was studied, and it was noted that a,w-dibasic acids and w-hydroxy-monobasic acids were the two dominated by hexadecane- I , 16-dioic acid and 16-hydroxyhexadecanoic acid as the major constituents in the suberin monomers of the bark of this species [ 1 l ] . Besides these acids, smaller amounts of long-chain primary alcohols, alkanoic acids, and ferulic acid were observed in C. libani bark, as are often observed with other species. Thus, the composition of the suberin monomer of the C. libnni bark was quite different from that of spruce and pine, where unsaturated C,,-acids (hydroxyoctadecenoic acid and octadecenedioic acid) were major monomers [ l ] . There were trials to isolate suberin from the bark without chemical action. Perra et al. extracted lignin and suberin from bark of Fngus sylvaticcr milled in a vibratory ball
246
Sakai
mill by extraction withaqueousdioxaneand purified each fraction. Treatment of the suberin fraction with BF,-methanol provided methyl esters of ferulic acid in addition to ordinary suberin monomers [12]. Preextracted corks from Quercus suber were thoroughly depolymerized by using a sodium methoxide-catalyzed methanolysis to detect 5.2% glycerol, 48.0% suberinic fatty acids and minor amounts of ferulic acid. A very mild depolymerization using calcium oxide-treated methanol solubilized only 2.0% of the cork material, of which43.8%were aliphatic acids, 2.1% werel-alkanols,and32.1%were monoacylglycerols. Based on GC-MS analysis of these acids and acylglycerols, Garqa and Pereira proposed that suberin is a glyceryl-based polymer and that its insoluble character is given, at least in part, by the cross-linking of dicarboxylic fatty acids with glycerol [ 131. In an alkaline extract of Pinus radiata bark, a,w-dibasic acids were found, suggesting that partial saponification of cutin or suberin occurred in the bark during the extraction [ 141. Dioxane-HC1 lignins of woods and barks of P. sylvestris and P. caribaea were studied comparatively. In both species the bark lignin showed smaller methoxyl contents and lower yields of vanillin upon nitrobenzene oxidation than wood lignin of the same species [9,15]. Thesebark lignin preparationsmusthavebeencontaminatedwith parts of condensed tannins which were resistant to extractions with neutral solvents and aqueous alkali.
IV.BARKEXTRACTIVES
Generally, bark contains much larger quantities of extractives than wood of the same tree, as seen from Table 1. Bark chemical components can be roughly fractionated by a sequence of extractions starting with a nonpolar solvent, such as petroleum ether, in many instancesfollowed by diethyl ether, ethanol, and water. Lesspolarcompoundssuchas waxes, resin, lipids, higher fatty acids, phytosterols, and terpenes are extracted mainly with non- or less polar solvents. On the other hand, ethanol and water dissolve relatively polar substances, such as flavonoids, phenolics, their glycosides, condensed tannins, sugars, etc. Acetone-water mixture is the preferred solvent for extraction of condensed tannins [ 15b]. Ethyl acetate is sometimes used for extraction of low-molecular-weight tannins or oligomeric proanthocyanidins. Aqueous NaOH solutions (e.g., 1%) have been often used for extraction of polymericcondensed tannins. However, attention should be given to the alkaline rearrangement resulting in partial or total rearrangement of tannins of the procyanidin class to “phenolic acid,” which have less phloroglucinol functionality [ 161. Saponification of ester bonds in cutin and suberin can also occur in aqueous alkali [ 141. The yields of sequential extracts from barks were compiled as tables by Laks [ I ] for various softwood tree species: Pseudotsuga menziesii, Pinus tueda, P. echinattr, l? virginiana, P. elliottii, P. sylvestris, P. brutia, l? btuksiana, P. corltortu, P. nigru, P. hulepensis, l? radiata,Piceueizgelnmnni, P. abies,Larixkaempferi, L. eurolepsis, L. deciducr,Abies balsurrtea, and Tsuga canadensis. Also compiled are the yields from barks of some hardwood species: Bruguierugymrtwrrhi:a.Rhizoplzera stylosa, Fugus sylvutica, Betula verI ’ U C O S ~ I ,B. allegl~uniensis,B. papyrifera, A1rur.s rubra, Populus tremuloides, Quercus d b a , and Q. rubra. Extractives yields recently published for barks of some species are listed in Table 2. The extractives content can vary according to a number of factors, including environmental, genetic, and seasonal variations. Seasonal fluctuation of extractive contents was investigated with barksof Quercus rohur; Piceacrbies, and Pirius.sdvestris grown in Germany [ 171. No season-related differences were observed in the amount of cyclohexane extract. Amounts of ethanol extract, NaOH cxtract,and water extract increased to different
rk
Chemistry of Bark TABLE 2
247
Yieldsof Extractives from Tree Barks Solvent Total
Hot
Species Hexane Benzene Ethanol water Ether 2.2-3.4 10.5-12.6 20.0-25.6 0.8-1.0 2.0-6.6 1.8-2.9h 3.2-5.1 0.5-0.8
Pinus pinastrr glohulus Eucalyptus Qurrcus rohrrr
Inner Outer bark radiata Pinus Cedrus
13.6
1 .9’
2.7
1.Od23.8‘ 2.9’
3 3
10.5
6.3 1 2.9h
1% NaOH
extractives Ref. 41.8
I61
-
6.3-8.5
[4]
14.0
40.0
[l71 1171
-
36.6
1181
[l91
“Hexane extract + benzene extract. hBenzene-ether. ‘Cycrohexane. “Toluene. ‘Ethyl acetate. ‘Acetone extract + MeOH extract. ’Petroleum ether. “Acetone.
extents from spring to winter. Of the three extracts, an increase in ethanol extract content was the most extensive. The extractives yield also depends on the aging between felling the tree and carrying out the analysis. Tree age influences the quantity and quality of bark extractives. In freshly cut P o ~ ~ u l u s t r m u r l o i d e sthe , higher up the tree,thegreater the amounts of bark extractives, probably due to the fact that the more inner bark regions are towards the top of the tree [ 201. Young Pinus rtrdiata bark (12 years old) provided extractives in a significantly higher yield (32.9%) than that (29.4%) from 30-year-old bark of the same species [2l]. In the case of Rhizoplzoru mucmmta, however, barks of older trees gave higher extractives and tannin contents [22].
A.
Lipophilic and Terpenoid Extractives
Waxes from Douglas fir bark were used for many purposes in the United States for several years from the late 1970s to the early 1980s. Thus,considerableknowledge has been accumulated on conifer bark waxes. Laks [ l ] cited such studies and listed major components of hydrolyzed and nonhydrolyzed bark waxes appearing in the literature until 1985. Free fatty acids, resin acids, and alcohols found in tree barks were also shown in a table. Little work has been performed on the lipophilic constituents of bark since1986. Analyses of sterol and wax esters in the “hexane wax’’ from Douglas fir (Psrudorsugcr ttzm:ie.sii) bark has revealed that the sterol ester was composed of sitosterol and campesterol esterified t o any or a l l of the fatty acids, C,,-, C,,-, C,,-, C,<,-.C?,!-, C??-, and C?,saturated acids. and oleic acid. The wax ester afforded, upon saponification, I-docosanol and I-tetrncosanol in addition to the above-mentioned fatty acids [23]. An ester mixture composed of such alcohols esterified to ferulic acid was isolated from bark hexane wax of the same species 1241. This mixture of a great number of individual esters is likely to account in part for the softness and low melting point of Douglas fir wax, ;IS Lavnr ct a l . I23 1 suggested.
Sakai
248
In petroleumetherextractivesof Cedrus libani bark, fatty acids, resin acids, and unsaponifiables occurred in similar amounts (35.4%, 34.3%, and 30.3%, respectively) [ 191. Compositionof the extractives after saponification is shown in Table 3. The saturated acidswerepredominantly fatty acids,similartobarkwaxes of manyotherconiferous species. Isopimaric acid was the principal constituent, while pimaric acid was not detected in the resin acids of the C. libani bark extractives. Fatty alcohols formed a dominating group in the saponifiable fraction, and tetracosanol was the main constituent of unsaponifiables. Normal paraffins from C,, to C,,) occurred in small amounts. Undec- IO-en-2-one and tridec- 12-en-2-one were identified as the major and minor components of the essential oil of the fresh bark of the Litseaelliptica tree, which is known for its termite resistance and repellent properties [3]. Examples of some mono-, di-, sesqui-, and triterpenes, and the species in which they occur, were shown by Laks [l]. Mono- and sesquiterpenes were recently identified in the essential oil of Magnolia oflcinalis bark, which has been used as a remedy for flatulent dyspepsia, cough, and asthma in China. By analysis with gas chromatography/mass spectrometry fitted with accurate mass analysis, 93.8% of the compounds detected in the oil were identified [25]. Thepredominantconstituentsweresesquiterpenes,P-eudesmol 17.4%, cadinol 14.670, and guaiol 8.7%. Their structures are shown in Fig. 2 . Glucosylated monoterpenic and sesquiterpenic tropolones wereisolated from the bark of Italian cypress, Cupressus senzpervirens, in response to infection by the fungus, Diplodia p i m a f. sp. cupressi. These tropolone glucosides inhibited in-vitro germination of spores
TABLE 3 Composition (%) ofPetroleumEtherExtractives from the Bark of Cedrus Iihani After Saponification [ 191
35.4 Resin acids Fatty acids Sandaracopimaric 0.5 Myristic Levopimaric 2.4 Palmitic Plustric 14-Methylhexadecanoic 0.9 0.4 Isopimaric Stearic Abietic 7.6 Oleic Dehydroabietic 1.1 5,9-Octadecadienoic Neoabietic 3.4 Linoleic Abietatrienic 0.9 Pinolenic Linolenic 0.5 Unsaponifiables Alkanes (C,?-C,,,) Arachidic I .3 Fatty alcohols 1 I , 14-Eicosadienoic I .2 Stearyl Behenic 3.6 Nonadesyl 7.1 Lignoceric Arachidyl Hexacosanoic 2.0 Behenyl Others 2.5 Lignoceryl Ceryl Phytosterols Campesterol Campestanol p-Sitosterol p-Sitostanol Others
34.3 1.0 0.9 6.3 9.8 4.9 5.7 5.3 0.4 30.3 1.S 18.3 0.4 0.9 I .3
2.1 2.2 11.4 8.4 2.6 0.2 5.1 0.5 2.1
249
Chemistry of Bark
a-Cadinol FIGURE 2
I)-Eudcsmol
Guaiol
Structures of cadinol, eudesmol, andguaiol
of various phytopathogenic fungi such asD.Pinecr, Seireciium cardinale [26]. A compound, (5aRY,6R*,9R*,9aS)-4-cinnarnoyl-3,6-dihydroxy1 -methoxy-6-methyl-9-( 1-methylethyl)5a,6,7,8,9,9a-hexahydrodibenzofuran(Fig.3),which is biosynthesizedprobablyfroma menthane type monoterpene and a chalcone, was isolated from the bark of Lindercr umhellatcr. This compound exhibited potent inhibitory activity on melanin biosynthesis [27]. Taxol, a unique and complex diterpenoid containing the taxane ring system, a rare four-memberedoxetane ring andestersidechains(Fig. 4), hasbeen one of the most extensivelystudiedditerpenoids in this decade. It was isolated as the majorcytotoxic principle in extracts from the bark of Pacific yew, R x u s brev$olin, by Wani et al. [28], but clinical trials were delayed. Phase I trials in human cancer commenced in 1983 and the great promise of taxol was confirmed. It has become an important new cancer chemotherapeutic agent, having significant activity in drug-refractory ovarian cancer. Taxol was approved for treatment of this disease by the U.S. Food and Drug Administration in 1992 [29]. Chemicalsynthesis[30],semisynthesisfromprecursors[31],production by endophytic fungi [32], and productionby cell cultures of Taxus spp. [33] have been studied very actively, since taxol is contained in different parts of Tuxus trees only in small amounts(Table 4) [34] and the trees grow quite slowly in general.Two new taxane diterpenoids (Fig. 4) were isolated from the barks of Taxus yunnanensis recently [35]. Diterpenoids with a daphnane skeleton (Fig. 5 ) were isolated from the bark of Wikstroemia retusa, which is used locally in the Ryukyu Islands in Japan for the preparation of traditional paper that can be stored for long periods of time, probably due to constituents against insect damage [36]. Daphnane diterpenoids have biological activities, e.g., antileukaemic, piscicidal, and antifertility. Three new pterocarpane-type diterpenes, margolone, margolonone, and isomargolonone, shown i n Fig. 6, were isolated from the stem bark of Azadirachta inclica (Meliaceae),
250
Sakai AcO
FIGURE 4
RA
Structures of taxol and some taxane diterpenoids obtained from bark of Erxus spp.
TABLE 4 Contents of Taxol in Different Parts of Trrrus Trees 1341 Plant Species 7irxus hrevifolicr
7: bncc.nrtr
7: rnrdin
7: ctrspicltrtcr
Taxol material Bark Roots Wood Wood with bark Branches Leaveslneedles Twigs Seedlings Stem Twigs Leaf Stem Twigs Leaf Twigs
(%)
0.015
0.004 0.0006 0.0003 0.00 17 0.00 1S 0.0012 0.0058 0.00 1 0.0006 0.003 0.002 0.009 1.002 0.0006
251
Chemistry of Bark R‘
R
R=HZ,R’=Mc,R”=COOH Margolonc R=O, R=Mc, R”=COOH Margolonone lsomargolononc R=O, R’=COOH, R”=Me FIGURE 6 Diterpenoids from the stem bark of Azcldirachfn indica.
which is regarded as a bitter tonic, astringent, and as being useful in fever, thirst, nausea, vomiting, and skin diseases [37]. These diterpenoids possessed different antibacterial activities against Klebsiella oxytoca, Staphylococcus epidermidis, and Serratia lutea. Supercritical carbon dioxide was used to extract cis-abienol efficiently from the bark of Abies saccharinensis [38]. This extract has a tobacco odor and oviposition-deterrent activity to some aphids and worms. Betulinand related triterpenes with the lupaneskeletonarecommon in barks of Betula species. Theirstructures are shown in Fig.7. However, their contents are very different from species to species, as shown in Table 5 [ 1,39-411. White-barked birches, B. verrucose in Europeand B.plutiphyllcr var. japonica in Japan,contained betulin to about 25% of their outer bark weight. On the other hand, much less betulin was observed in the barks of dark-barked birches, B. ermani in Japan and B. nigrll in North America. Especially in the latter species, betulin and lupeol were no longer the predominant triterpene components, and 3-O-acetyloleanolic acid predominated [40]. Triterpene contents in inner bark and root bark were very much smaller than those in outer bark. It is noteworthy that all the triterpenes isolated were caffeoylated in the root bark of B. ermcmii [41]. Betulin oligosaccharides were enzymatically synthesized by using cyclodextrin glycosyl transferase withan aim to increase its biological activity [42].Unsaponifiables in the barks of Fclgus crenata, Cyclobanopsis glauca, and Castanopsiscuspiciata wereclaimedtobe responsible for “pitch trouble” during kraft pulping process, as lots of pitch specks were observed on pulp sheets prepared from wood chips contaminated with their barks. These barks have larger contents of unsaponifiables than wood 1431.
B.
Low-Molecular-WeightPhenolics
Laks [ l ] dealt withlow-molecularphenolicextractivesincluding flavonoids, lignans, phenylpropanoids,andothersimplephenolicsfound i n tree barks until 1985and cited somereviewsandbooksconcerningthem. In this section onlymore recent results are referred to. Phenolic compounds are present in relatively large amounts in coniferous tree barks. Thebarks of somehardwoodspecies,such as Q w m l s , Euctrlyptus, Accrcicl. and Soli.v, also contain large amounts of phenolic extractives, as exemplified in Table 6, while some of otherhardwoodspecies, Betulcl spp., for instance, containonly negligible amounts of phenolic extractives in their outer barks. Itis likely that phenolic constituents i n the
252
Sakai
CH,OH CH 2OH CH0 CO2H CO2Mc CO ?H C02Mc CO 2H CH3 CH 3 CH3 CH0
AC:
CH,C&
FIGURE 7 Structures of' triterpenes found in Betlrlcr barks.
inner bark and root bark are largely glycosylated so that they can be translocated in the phloem sap.
1. Monoaryl Compounds, Lignans, andRelated Products A variety of phenolic compounds has been found in bark, as described by Laks i n the first edition of this volume I l]. Common natural products with a phenylnlethane (C,-C,)skel-
etonare the hydroxylated benzoic acid and benzaldehydederivatives which have been found in many plant materials including barks of many softwood and hardwood species. A recent example in this regard is an HPLC evaluation of Elrcalyfrrs glohulus bark, which
Chemistry of Bark
253
TABLE 5 Triterpenoid Composition in the Barkof Betula spp.
Composition (% of the bark) B. vrrrrcosa
[I1
Compound (structures in Fig. 7) Betulin (=Beturinol) (1) 3-0-caffeoylbetulin (2) Betulinic aldehyde (3) Betulinic acid (4) + methyl betulinoate (5) 3-0-Acetylbetulinic acid (6) Methyl 3-0-acetylbetulinoate (7) 3-0-caffeoylbetulinic acid (8) Lupeol (9) 3-0-caffeoyllupeol (10) Lupenone (11) Lup-20(29)-ene-3-one-28-al(12) Oleanolic acid (13)
3-0-Acetyloleanolic acid (14) 3-0-Caffeoyloleanolic acid (15) 3-P-Acetoxyolean-I 1-oxo- 12-ene28-oic acid (16) Monogynol (17) 3-0-Caffeoyldammarendiol I1 (18)
Others
0
B. phtyphylla var. jnponicc~ B. nigra ~ 9 1 l401
B. ermanii [41]
0
0
0
I”
26.20
0.134 0.067
3.515
-
0.030
-
-
-
-
-
0.011 -
1.34 -
-
0.03 0.96
0.010 0.006 -
-
-
-
0.01 1
1.oo 0.14 -
0.038
0.07
-
R
0.062
0.129 0.462 0.015 0.02 1
-
“0,1, and R denote outer bark, inner bark, and root bark, respectively. hIncludes methyl oleanolate and 3-0-acetyloleanolic acid.
revealed the presence of gallic, protocatechuic, vanillic, and ellagic acids, and protocatechuic aldehyde, together with some flavonoids and ellagitannins [46].Some ellagic acid derivatives, methylated and/or glycosylated, were isolated from the stem bark of Diplopanax stachvanthus [47]. The bitter-tasting bark of Prunus gra-yancl contains phenylethanoid (C,-C,) glucosides and their caffeate esters, together with a tannin-related 3,4,S-trimethoxybenzoyl-glucoside. The latter two had a strong bitter taste [48].Arylpropanoids (C,-C,) biologically synthesized from the amino acid phenylalanine are very common in the plant kingdom and are constituents of the naturally important phenolic polymers, lignins and condensed tannins. Arylbutanoid (C,-C,) glycosidesareknowntobe present in the inner bark of Betula pendula 1491 and in the stem bark of A c e r nicoense [SO]. Bioactive styryl-lactones, goniofufuranone, goniopypyranone, and 8-acetylgoniotriol (Fig. 8) were isolated from the stem bark of Goniothalarnus giganteus [Sl]. Thesecanberegarded as phenylheptanoids (C,-C,). Isorhapontin, one of the stilbenes (C(,-C2-C,),was found to be present in very high content (13%) in the bark of Picea engelmanni. This content was dramatically different
I
Sakai
254 TABLE 6
Contents of Phenolic Extractives in Barks 70% acetone extracts
Total phenolics
Plant name
(%)
(%)
S. roricln S. kinrcyanagi 13.7
34.9 30.0 31.0 27.2
17.2
13.2 S. gilgiana S. grncilistda 12.9 Run1e.r hastotus Acncicrniloticcc 21.3 A. auriculiformis A. fcrrnesiana 18.7 A. leucophloecl A. ferruginecc4.6 A. torta 4.6 A. ctresicr 6.6 A. srtrldnr A. dedbcrta 14.0 A. larronutn 15.3 Bruguiern gymnorrhiza ' 13.1 B. gytlrrorrhizrc h Ceriops tcrgrcl"45.2 Rhizopharc~apiccclcrtcr 19.3 '' R. rnucro~ntrtrr" 29.4 R. stylosoh 26.2 35.2 Xylocccrpcs grcrncrtutn 17.9 Sorrtrernticr cclhcr"
Tannin content
(a)
(%l
Ref.
17.7
9.7 7.7 9.0 5.6
[101
15.0
-
16.8 11.8 10.4
14.4 9.9
33.8 25.8 35.5 25 .o 13.3 19.6 24.7
1451 - [45 -
17.2 13.2
3.O
9.5
21.7 36.9 22.8 24.8 45.8 28.4 41.8 32.6 35.9 24.2
Total flavanols
t451 13.9
t651
-
9.9 30.7 25
[651
21.9 25
[ 101
[101 [ 101
1441 19.2 15.8 15.4 12.8 3.7 4.1 6.2 2.6 13.3 12.3
12.0 8.8 35.4 15.1 (651 24.4 22.2 27.6
10.0
15.5
13.8
t451
1451 1451
1 1451 [451
1451 1451 1651 1651
12.4
.o
1651
.o
t651 1651
"Grown in Thailand. hGrowninJapan.
from those in other softwood barks from five genera, suggesting isorhapontin to be a good taxonomic marker [S2]. Phenyl propane dimers (C&,-C$,) linked at the P-positions are referred to as lignans, and ones linked at a position different from the P are sometimes called neolignans. A book of lignans in general [S31 and a review of lignans from woody plants [S41 was published recently. In the root bark of A c c r n / / ~ r ~ ~ ~ r rsrn/ico.su.s, nc~x an empiricaloriental medicinal plant. five lignans, two coumarins, and three other phenolic compounds were
Gonyofufuronc FIGURE 8
Goniopypyronc
Structures o f biouctive styryl-lactoncs.
X-Acctylconiotriol
Chemistry of Bark
255
identifed. Seven of these compounds were glycosides and one was caffeate. The predominant constituent was syringaresinol diglucoside 1551. A neolignan rhamnoside and a lignan xyloside were isolated from the inner bark of Ostrya japonica [57]. Betula ermanii inner bark contains two lignan glycosides and a dicaffeoylated lignan [41]. Contents of lignans were compared between the wood and bark of Magnolia kobus var. borealis, which has been used as a material for Oriental medicine blends [58].The bark contained much larger amounts of lignans, especially permethylated lignans, magnolin, and yangambin. The bark of Ocotca catharinensis contains I O neolignans(average yield 0.07%) of thebicyclo[3.2. lloctanoid and the hydrobenzofuranoid structural types [59]. These neolignans are also present in much larger contents in the bark than in wood of the same species. A series of diarylheptanoid (C,-C,-C,) glycosides together with the aglycon, platyphyllone, was identified in the inner bark of Betula pendula [49], and a diarylheptanoid glycoside platyphylloside was found to be present at high levels in B. pendula (20-60 mg/g dry bark) but at low levels in B. pubescens (
2. Flavonoids and Proanthocyanidins Barks of almost all tree species contain flavonoids with carbon skeleton C,-C&, (Fig. 9). The first edition [ l ] dealt with somecommon flavonoids includingquercetin,dihydro-
R5
R5
Catechin(CAT)
2R :3s
H
Epicatcchin (ECT)
2R:3R
OH
H OH OH OH OH H
ent-Catechin (entCAT)*
2S:3R
OH
H
Galloatechin (GCT)
2R : 3 s
OH
Fisetinidol (FIS)
2R :3s
H H
Robinctinidol (ROB)
2R :3s
H
OH OH OH OH OH OH
OH OH OH OH OH OH OH OH OH
H H
H OH OH OH OH
OH OH OH OH OH
H
FIGURE 9 Basic structure, numbering system, and configuration offlavonoids flavan-3-01s). *Use the right structure for ent-flavan-3-01s.
(exemplifiedfor
I
Sakai
256
quercetin,myricetin,and their glycosides found in the bark. After that, some excellent reviewsandbooksonflavonoids and related compoundswerepublished[15b,66,67], though they are not confined to the bark components. The flavan-3-01s catechin and epicatechin are very commonly present in the bark, probably as precursors to and by-products of the biosynthesis of condensed tannins. Flavan-3-01 glycosides were thought to be rare. However, some were recently found in the inner bark of different species, for example, catechin 3-O-a-~-rhamnopyranosidein Quercus miyagii bark [68]. catechin 3-o-p-D-ghcopyranoside and 3-O-[au-~-rhamnopyranosyl-( 1 +6)-P-~-gulucopyranosyl]-catechin in Quercus marilandica bark 1691, and catechin 7-O-~-D-glucopyranosidein the inner barks of Betula pubescens 1701 and Pseudotsugu menziessii [71]. The latter also contained epicatechin 7-O-p-D-glucopyranoside, catechin 4'-O-P-~-glucopyranoside, and 3'-O-methylepicatechin 7-0-P-D-glucopyranoside as flavan-3-01 glycosides [71]. The position 3 of the flavanols is sometimes gallo