This Page Intentionally Left Blank
NGUYEN
QUANG
MINH
ALLIEDSIGNAL, INC. AEROSPACE EQUIPMENT SYSTEMS TORRANCE, CALI...
182 downloads
2908 Views
14MB Size
Report
This content was uploaded by our users and we assume good faith they have the permission to share this book. If you own the copyright to this book and it is wrongfully on our website, we offer a simple DMCA procedure to remove your content from our site. Start by pressing the button below!
Report copyright / DMCA form
This Page Intentionally Left Blank
NGUYEN
QUANG
MINH
ALLIEDSIGNAL, INC. AEROSPACE EQUIPMENT SYSTEMS TORRANCE, CALIFORNIA, U.S.A.
T A K E H I KO T A K A H A S H I PROFESSOR EMERITUS NAGOYA UNIVERSITY NAGOYA, OAPAN
1995 ELSEVIER AMSTERDAM
9 LAUSANNE
9 NEW
YORK
9 OXFORD
9 SHANNON
9TOKYO
ELSEVIER SCIENCE B.V. Sara Burgerhartstraat 25 P.O. Box 2II, IOOOAE Amsterdam, The Netherlands
Library
of Congress C a t a l o g i n g - i n - P u b l i c a t i o n
Data
Nguyen, Quang Minh. Science and t e c h n o l o g y of ceramic f u e l c e l l s / Nguyen Quang Minh, Takehiko T a k a h a s h i . p. cm. Includes bibliographical r e f e r e n c e s and index. ISBN 0 - 4 4 4 - 8 9 5 6 8 - X 1. S o l i d oxide f u e l c e l l s . I. Takahashi, Takehiko. II. Title. TK2931.N48 1995 621.31'2429--dc20 95-21137
CIP
ISBN: o 444 89568 X 9 I995 Elsevier Science B.V. All rights reserved. No part of this publication may be reproduced, stored in a retrieval system or transmitted in any form or by any means, electronic, mechanical, photocopying, recording or otherwise, without the prior written permission of the publisher, Elsevier Science B.V., Copyright & Permissions Department, P.O. Box 52i, zooo AM Amsterdam, The Netherlands. Special regulations for readers in the U . S . A . - This publication has been registered with the Copyright Clearance Center Inc. (CCC), 222 Rosewood Drive, Danvers, MA 01932. Information can be obtained from the CCC about conditions under which photocopies of parts of this publication may be made in the U.S.A. All other copyright questions, including photocopying outside of the U.S.A., should be referred to the publisher. No responsibility is assumed by the publisher for any injury and/or damage to persons or property as a matter of products liability, negligence or otherwise, or from any use or operation of any methods, products, instructions or ideas contained in the material herein. This book is printed on acid-flee paper. Printed in The Netherlands.
Dedicated to my late father, Mr. Nguy~n Du~ N.Q.M.
Dedicated to my wife, RiO Takahashi T.T.
This Page Intentionally Left Blank
PREFACE
Ceramic fuel cells, commonly known as solid oxide fuel cells (SOFCs), have been under development for a broad spectrum of electric power generation applications. The most attractive feature of the SOFC is its clean and efficient production of electricity from a variety of fuels. The SOFC has the potential to be manufactured and operated cost-effectively and, thus, promises to be an important alternative source for generating electric power in the future. At present, SOFC technology is still in its development stage, and several technical challenges remain to be resolved before the fuel cell becomes a fullfledged, practical power system. In the past several years, SOFC technology has received much attention. Development effort in this area has expanded significantly, and the number of conferences and publications on SOFCs has increased dramatically. The widening interest in this technology arises, in part, from the continuing need to develop cleaner and more efficient means of converting energy sources into useful forms. Recent advances in ceramic technology, especially in synthesizing fine powders, engineering material compositions, tailoring composition/property relationships, and processing intricate structures, have also contributed to the increased interest in SOFCs. These technological advancements have led to improved designs, better performance, and cost-effective manufacturing methods. As a result, significant progress toward practical applications of the SOFC has been made. This book has been written to provide a comprehensive treatise on SOFCs and to fill the need for a reference book on the technology. It is directed toward scientists, engineers, and technical managers working with SOFCs, ceramic devices based on conducting materials, and in related fields such as solid-state ionics and electronic ceramics. The book can also be used as a text for science and engineering courses at the senior or graduate level. As the field of SOFCs is still evolving, this book has been prepared with an emphasis on the discussion of known facts and reported experimental data. Dated information has been kept to a minimum; however, in some instances, this type of information was included to give insights into work now in progress and to provide guidance
viii
Preface
for future work. It is possible that some ideas and explanations discussed in the book may change as the technology progresses. We greatly appreciate the encouragement and support of many colleagues during the writing of this book. We are grateful to Ms. Lynn Silver for her editorial assistance.
Torrance, California, USA Nagoya, Japan December 1994
9 NGUYEN QUANG MINH TAKEHIKO TAKAHASHI
CONTENTS
Chapter 1
INTRODUCTION 1.1 1.2
Scope, 1 General Characteristics of Ceramic Fuel Cells, 3 1.2.1 Types of Ceramic Fuel Cells, 4 1.2.2 Cell Components, 6 1.2.3 Comparison with Other Types of Fuel Cells, 10 1.3 Historical Background of Ceramic Fuel Cells, 10 References, 14
Chapter 2
PRINCIPLES OF OPERATION
15
2.1 2.2 2.3
General, 15 Thermodynamic Principles, 16 Fuel Cell Efficiency, 20 2.3.1 Electrochemical Efficiency, 21 2.3.2 Other Efficiencies, 24 2.4 Power Generation, 25 2.5 Characteristics of Ceramic Fuel Cells, 28 2.5.1 Features, 28 2.5.2 Effect of Electronic Conduction in Electrolyte, 29 2.6 Types of Fuel and Oxidant, 36 2.6.1 Fuel, 37 2.6.2 Oxidant, 38 2.7 Fuel-Processing System, 38 2.8 Power-Conditioning System, 39 References, 40
Chapter 3
ELECTRICAL CONDUCTION IN CERAMICS 3.1 3.2
General, 41 Defects in Fluoride-Type Oxides, 43 3.2.1 Defect Structure of Doped MO2, 44 3.2.2 Conductivities of Oxygen Ions, Electrons, and Electron Holes, 50 3.2.3 Defect Domains, 52 3.2.4 Defect Associations and Clusters, 54
41
x
Contents
3.3 3.4
Defects in Perovskite-Type Oxides, 56 Conduction Processes and Transference Numbers, 60 3.4.1 General Transport Equations, 60 3.4.2 Electronic, Ionic, and Total Current, 61 3.4.3 Transference Number Measurements, 62 References, 67 Chapter 4
ELECTROLYTE
69
4.1 4.2
Requirements, 69 Stabilized Zirconia, 70 4.2.1 Preparation, 71 4.2.2 General Properties and Phase Transformation, 74 4.2.3 Stability, 76 4.2.4 Electrical Conductivity, 78 4.2.5 Chemical Interaction, 87 4.2.6 Thermal Expansion, 87 4.2.7 Mechanical Properties, 90 4.3 Doped Ceria, 92 4.4 Stabilized Bismuthsesquioxide, 96 4.5 Other Oxygen-Ion Conductors, 101 4.6 Protonic Conductors, 102 References, 107 Chapter 5
CATHODE
117
5.1 5.2
Requirements, 117 Lanthanum Manganite, 118 5.2.1 Preparation, 118 5.2.2 General Properties, Phase Transformation, and Stoichiometry, 120 5.2.3 Stability, 126 5.2.4 Electrical Conductivity, 127 5.2.5 Chemical Interaction, 132 5.2.6 Thermal Expansion, 135 5.2.7 Other Properties, 137 5.3 Lanthanum Cobaltite, 138 5.4 Other Materials, 139 References, 140 Chapter 6
ANODE 6.1 6.2
Requirements, 147 Nickel/Yttria-Stabilized Zirconia Cermet, 148
147
xi
Contents
6.2.1 Preparation, 149 6.2.2 Stability, 153 6.2.3 Electrical Conductivity, 156 6.2.4 Chemical Interaction, 158 6.2.5 Thermal Expansion, 159 6.3 Other Materials, 160 References, 161
Chapter 7
INTERCONNECT
165
7.1 7.2
Requirements, 165 Lanthanum Chromite, 166 7.2.1 Preparation, 166 7.2.2 General Properties, Phase Transformation, and Stoichiometry, 168 7.2.3 Stability, 171 7.2.4 Electrical Conductivity, 172 7.2.5 Chemical Interaction, 180 7.2.6 Thermal Expansion, 181 7.2.7 Sinterability, 183 7.2.8 Gas Permeability, 188 7.3 Other Materials, 188 References, 191
Chapter 8
ELECTRODE REACTION
199
8.1 8.2
General, 199 Reactions at Anode, 200 8.2.1 Electrochemical Oxidation of Hydrogen, 200 8.2.2 Electrochemical Oxidation of Carbon Monoxide, 208 8.2.3 Reaction of Sulfide Impurities, 209 8.2.4 Reforming of Hydrocarbons, 210 8.3 Reactions at Cathode, 212 8.3.1 Oxygen Reduction at Metal Electrode, 214 8.3.2 Oxygen Reduction at Oxide Electrode, 216 References, 225
Chapter 9
STACK DESIGN AND FABRICATION 9.1 9.2
General, 233 Sealless Tubular Design, 235 9.2.1 Design Features, 235 9.2.2 Advantages and Disadvantages, 239 9.2.3 Fabrication, 240
233
xii
Contents
9.2.4 Performance and Technological Status, Segmented-Cell-in-Series Design, 255 9.3.1 Design Features, 255 9.3.2 Advantages and Disadvantages, 259 9.3.3 Fabrication, 260 9.3.4 Performance and Technological Status, 9.4 Monolithic Design, 268 9.4.1 Design Features, 268 9.4.2 Advantages and Disadvantages, 270 9.4.3 Fabrication, 272 9.4.4 Performance and Technological Status, 9.5 Flat-Plate Design, 282 9.5.1 Design Features, 282 9.5.2 Advantages and Disadvantages, 287 9.5.3 Fabrication, 287 9.5.4 Performance and Technological Status, References, 297
252
9.3
Chapter 10
266
280
293
MODELING AND ANALYSIS
307
10.1 General, 307 10.2 Stress Analysis, 308 10.3 Electrical Analysis, 314 10.4 Modeling of Current and Temperature Distribution, 321 References, 328 Chapter 11
SYSTEM AND APPLICATION
331
11.1 General, 331 11.2 Electric Utility, 332 11.3 Cogeneration, 335 11.4 Transportation, 338 11.5 Space and Other Applications, 343 References, 347 Appendix. Selected References Relevant to Solid Oxide Fuel Cell Technology 351 Reprint Permission
355
Index
357
Chapter 1 INTRODUCTION 1.1 SCOPE Fuel cells are a radically different way of making electrical power from a variety of fuels. A fuel cell is an energy conversion device that produces electricity (and heat) directly from a gaseous fuel by electrochemical combination of the fuel with an oxidant. Such a device bypasses the conversion of chemical energy of fuel into thermal and mechanical energy, and thus achieves theoretical efficiency significantly higher than that of conventional methods of power generation. In addition to the high conversion efficiency, fuel cells have the characteristics of environmental compatibility, modularity, siting flexibility, and multifuel capability. (i) High conversion efficiency: The primary feature of a fuel cell is its high fuel-to-electricity conversion efficiency (45 to 60%). A fuel cell converts the chemical energy of fuel directly into electrical energy. Thus, the usual losses involved in the conversion of fuel to heat, to mechanical energy, and then to electrical energy are avoided. The efficiency of a fuel cell is further improved when the byproduct heat is fully utilized (in cogeneration or bottoming cycles). (ii) Environmental compatibility: Fuel cells are capable of using practical fuels as an energy source with insignificant environmental impact. Emissions of key pollutants from fuel cells are several orders of magnitude lower than those produced by conventional power generators. Production of undesirable materials such as NOx, SOx, and particulates is either negligible or undetectable for fuel cell systems (for examples, see Figures 11.1 and 11.6, Chapter 11). (iii) Modularity: Fuel cells have the characteristic of modularity, i.e., cells can be made in modular sizes. Thus, fuel cell size can be easily increased or decreased. Since the efficiency of a fuel cell is relatively independent of size, fuel cells can be designed to follow loads with fast response times without significant efficiency loss at part-load operation.
2
Chapter 1 (iv) Siting flexibility:
Because fuel cells can be made in a variety of sizes, they can be placed at different locations with minimum siting restrictions. Fuel cell operation is quiet because a fuel cell has no moving parts; the only noises are those from auxiliary equipment. Consequently, fuel cells can be easily located near points of use such as urban residential areas. (v) Multifuel capability: Certain types of fuel cells have multifuel capability. High-temperature fuel cells can process (reform) hydrocarbon fuels internally and do not need expensive subsystems to process conventional fuels into simple forms. Ceramic fuel cells having the attributes discussed above are among the several fuel cell technologies being developed for a broad spectrum of electric power generation applications. The key characteristic of this type of fuel cell is its ceramic electrolyte. The use of a solid electrolyte in ceramic fuel cells eliminates material corrosion and electrolyte management problems and permits unique cell designs with performance improvements. The conductivity requirement for the ceramic electrolyte necessitates high operating temperatures (600 ~ to 1000~ High operating temperatures promote rapid reaction kinetics, allow reforming of hydrocarbon fuels within the fuel cell, and produce highquality byproduct heat suitable for use in cogeneration or bottoming cycles. On the other hand, high operating temperatures impose stringent material and processing requirements. The present key technological challenge facing ceramic fuel cells is the development of suitable materials and fabrication processes to incorporate materials into required structures. To date, although ceramic fuel cell technology is still evolving, it has made excellent technical progress. Multikilowatt fuel cells incorporating various features of a practical power generation system have been operated for thousands of hours and have shown excellent performance. Recently, ceramic fuel cell research and development has received much attention, reflecting widening interest in this technology. The objectives of this book are to provide a comprehensive treatise on both the fundamental and technological aspects of ceramic fuel cells and to serve as a reference source on this emerging technology. This book consists of eleven chapters. Chapter 1 introduces the general characteristics of ceramic fuel cells and gives a brief historical perspective on the development of this type of fuel cell. Chapter 2 provides an overview of the operating principles, with brief discussions on thermodynamic aspects of cell operation, key features of the fuel cell, types of fuel and oxidant, and other elements of a fuel cell power system.
Introduction
3
Since the operation of a ceramic fuel cell is based fundamentally on electrical processes in the ceramic components, it is instructive to outline some of the relevant theoretical considerations on electrical conduction in ceramics. Chapter 3 thus includes discussion on the general principles of electrical conduction, the relationships between conduction and defect structure, and transference numbers of ions and electrons in ceramics. Chapters 4, 5, 6, and 7 cover the principal components of a fuel cell stack: the electrolyte, the cathode, the anode, and the interconnect, respectively. Emphasis is given to the discussion on the preparation of each component material, its stability, and its chemical, electrical, and thermal properties under cell fabrication and operation conditions. Chapter 8 reviews various aspects of the electrode reactions, including reforming and contaminant reactions, in a ceramic fuel cell. The discussion in this chapter focuses on the reaction mechanisms of the hydrogen oxidation and the oxygen reduction. Chapter 9 is devoted to a thorough discussion of stack design and fabrication. Detailed description of design characteristics, gas manifolding, and fabrication processes, along with a summary of the technological status of each stack design, are presented. Chapter 10 provides a treatment of modeling and analysis used in ceramic fuel cell design, especially thermal stress analysis, electrical analysis, and performance modeling of various cell and stack configurations. Finally, the applications of ceramic fuel cells are discussed in Chapter 11. 1.2 GENERAL CHARACTERISTICS OF CERAMIC FUEL CELLS A ceramic fuel cell is an all-solid-state energy conversion device that produces electricity by electrochemically combining fuel and oxidant gases across an ionic conducting ceramic. A ceramic fuel cell consists of two electrodes (the anode and cathode) separated by a solid electrolyte. Fuel is fed to the anode, undergoes an oxidation reaction, and releases electrons to the external circuit. Oxidant is fed to the cathode, accepts electrons from the external circuit, and undergoes a reduction reaction. The electron flow (from the anode to the cathode) produces direct-current electricity (Figure 1.1) [1.1]. The solid electrolyte conducts ions between the two electrodes. Present ceramic fuel cells use exclusively hydrogen as fuel, and oxygen as oxidant. In theory, any gases capable of being electrochemically oxidized and reduced can be used as fuel and oxidant in a fuel cell. However, hydrogen is currently the most common fuel, since it has high electrochemical reactivity and can be derived from common fuels such as hydrocarbons, alcohols, or coal.
4
Chapter 1
FUEL~
ANODE ELECTROLYTE
, ox,o..
EXTERNAL LOAD
ANDHEAT/
CATHODE
Figure 1.1. Schematic diagram of fuel cell operation [1.1]
Oxygen is the most common oxidant, since it is readily and economically available from air. For the hydrogen/oxygenreaction, to date, only oxides are being considered for use as ceramic fuel cell electrolytes. Since fuel cells are commonly identified by the type of electrolyte used, ceramic fuel cells are referred to as solid oxide fuel cells (SOFCs). Due to the conductivity requirement for the oxide electrolyte, current SOFCs operate in the temperature range of 600 ~ to IO00~ 1.2.1 Types of ceramic fuel cells
A fuel cell electrolyte must ionically conduct one of the elements present in the fuel or oxidant. Thus, a solid electrolyte for SOFCs based on the electrochemical reactions of hydrogen and oxygen must conduct either oxygen ions or hydrogen ions (protons). (Although hydroxide-ion conduction is also possible, it has been shown to be a proton conduction with oxygen-ion carrier species. It is a special case and, for simplification,it will be considered as proton conduction here.) The present generation of ceramic fuel cells can be classified into two types [1.2]: (i) those based on oxygen-ion-conducting electrolytes and (ii) those based on proton-conducting electrolytes. Figures 1.2 and 1.3 show the reactions in an oxygen-ion-conductor SOFC and a proton-conductor SOFC, respectively. An oxygen-ion-conductor SOFC can be considered as an oxygen concentration cell, and a proton-conductor SOFC as a hydrogen concentration
Introduction
/
FUEL .... ~
0 H2C ' O/ ANODE +H20~C02+H2
,0=
"1 TO BURNE~/
//
~ / e ' . ~ "~ .... C O ~ ~ e - ~
,,THO0,
~EXCESS FUEL~
H2, CO. H20,C;2
1, / ~2 H~O.H20+C02
INTERFACE 0= + H2 ----~H20+ 2e-
02 + 4e-
5
"
e-
OUTER CIRCUIT
,,0:
~
)20=
132-t /
AIR OR 02
02/
|/ /
/
"
\
e"
02
CATHOD EXHAUST/
REACTION H2 + 1/202 ~-H2O CO + 1/202 = C02
Figure 1.2. Schematic diagram of reactions in SOFCs based on oxygen-ion conductors [1.1]
EXCESSFUER~
H2
/
FUEL H2 " ~
I / H2
ANODE H2 ~ 2H+ + 2e-
H~..... -e~''~' H+~je
!N_TERFACE_---~ 2H+ +I/202+ 2e--*H20
1
IH ~,
,H+
,
_
OUTER [, CIRCUIT
\r
CATHOOE 02
OXIDANT AIR OR 02
"-ITO BUR.NE
H20
,
HHo ! ,,..-
J
CATHOOE~
"-I EXHAUST
OVERALLREACTION H2 + V202~ H20
Figure 1.3. Schematic diagram of reactions in SOFCs based on proton conductors [1.1]
6
Chapter 1
cell. The major difference between the two SOFC types is the side in the fuel cell in which water is produced (the fuel side in oxygen-ion conductor cells and the oxidant side in proton-conductor cells). Also, certain gases, such as CO, can be used as fuel in oxygen-ion conductor SOFCs but not in proton-conductor SOFCs. To date, almost all of the development work on ceramic fuel cells has focused on SOFCs with oxygen-ion-conducting ZrO2 electrolytes. Work on proton-conductor SOFCs is limited to material studies, clarification of conduction mechanisms, and testing of small, laboratory-scale cells.
1.2.2 Cell components A SOFC single cell consists of an oxide electrolyte sandwiched between an anode and a cathode. Under typical operating conditions (with hydrogen fuel and oxygen oxidant), a single cell produces less than 1 V. Thus, practical SOFCs are not operated as single units; rather, they are connected in electrical series to build voltage. A series of cells is referred to as a stack. A component, variously called an interconnect or a bipolar separator, connects the anode of one cell to the cathode of the next in a stack (Figure 1.4). SOFC stacks can be configured in series, parallel, both series and parallel, or as single units, depending on the particular application.
INTERCONNECT
ANODE REPEATING ELEMENTS ELECTROLYTE
CATHODE
Figure 1.4. Fuel cell component
Introduction
7
The principal components of a SOFC stack are the electrolyte, the anode, the cathode, and the interconnect. Each component serves several functions in the fuel cell and must meet certain requirements. Each component must have the proper stability (chemical, phase, morphological, and dimensional) in oxidizing and/or reducing environments, chemical compatibility with other components, and proper conductivity. The components for ceramic fuel cells must, in addition, have similar coefficients of thermal expansion to avoid separation or cracking during fabrication and operation. The electrolyte and interconnect must be dense to prevent gas mixing, while the anode and cathode must be porous to allow gas transport to the reaction sites. The requirements for the various cell component are summarized in Table 1.1. In addition to the requirements listed in Table 1.1, other desirable properties for the cell components from practical viewpoints are high strength and toughness, fabricability, and low cost. Also, for certain cell designs, the components for a ceramic fuel cell must be amenable to limited fabrication conditions since the process conditions cannot be selected independently for each component. For example, if the components are built up one by one, the temperature of sintering for each successive component must be lower than that of the preceding component to avoid altering the microstructure of the preceding component. If the components are formed in the green state, then all components must be sintered under the same firing conditions. Furthermore, the components of a ceramic fuel cell must be compatible not only at the operating temperature but also at the much higher temperatures at which the ceramic structures are fabricated. Cell components are connected (in electrical series) in proper order in a stack. The height or number of single cells (thus, voltage) and footprint or active area (thus, current) of a stack can vary, depending on the particular design and power output required. Because all the components are solid, the SOFC stack can be configured into unique shapes unachievable in other types of fuel cells. At present, four common stack configurations have been proposed and fabricated for SOFCs: the sealless tubular design, the segmented-cell-in-series design, the monolithic design, and the flat-plate design (for more details, see Chapter 9). Each design may have several different versions and is presently at a different stage of technology development. Figure 1.5 shows, as an example, the schematic diagrams of the various SOFC stack designs [1.3].
TABLE 1.1 8
Requirements for Ceramic Fuel Cell Components
-
-
-
-
--
-
Requirements Component
Compatibility
Porosity
Thermal Expansion
Electrolyte
High ionic conductivity Negligible electronic conductivity
Chemical, phase, morphological, and dimensional stability in fuel and oxidant environments
No damaging chemical interactions or interdiffusion with adjoining cell components
Fully dense
Thermal expansion match with adjoining components
Cathode
High electronic conductivity
Chemical, phase, morphological, and dimensional stability in oxidant environment
No damaging chemical interactions or interdiffusion with adjoining cell components
Porous
Thermal expansion match with adjoining components
Anode
High electronic conductivity
Chemical, phase, morphological, and dimensional stability in fuel environment
No damaging chemical interactions or interdiffusion with adjoining cell components
Porous
Thermal expansion match with adjoining components
Interconnect
High electronic conductivity Negligible ionic conductivity
Chemical, phase, morphological, and dimensional stability in fuel and oxidant environments
No damaging chemical interactions or interdiffusion with adjoining cell components
Fully dense
Thermal expansion match with adjoining components
1
Stability
Chapter
Conductivity
Introduction
INTERCONNECTION
9
ELECTROLYTECATHODEINTERCONNECT'~~
ELECTRODE
/ ~ili \i : : Po.ouss0PPo.Ti: :::i: : : : : i : ,~.
I POROUSS
AIRFLOW
/
~
~-~~ FUELELECTRODE
ELECTROLYTE
~U )) ))'~ /) /)_) --" OXIDANT
Seal-less TubularDesign
-----e,
Segmented-Cell-in-SeriesDesign
ELECTROLYTE
Monolithic Design
Flat-plate Design
Figure 1.5. SOFC stack designs [1.3]
10
Chapter 1 1.2.3 Comparison with other types of fuel cells
The SOFC is one of several types of fuel cells currently under development for clean and efficient electric power generation from a variety of fuels. Besides the SOFC, the other major types of fuel cells are polymer membrane, alkaline, phosphoric acid, and molten carbonate fuel cells. Among these fuel cells, the phosphoric acid fuel cell is presently at the initial stage of commercialization for electric utility and cogeneration uses. The molten carbonate is the next most likely candidate for commercialization, whereas the SOFC is considered as the third-generation technology. The polymer membrane fuel cell is being developed mainly for space and transportation applications, and the alkaline fuel cell is an important power source for space flights. Typical features and operational characteristics of the SOFC and other types of fuel cells are listed in Table 1.2. 1.3 HISTORICAL BACKGROUND OF CERAMIC FUEL CELLS The principles of fuel cell operation were first reported by Sir William Grove in 1839 [1.4]. His fuel cell used dilute sulfuric acid as the electrolyte and operated at room temperature. Ceramic fuel cells came much later and began with Nernst's discovery of solid-oxide electrolyte in 1899 [1.5] and the operation of the first ceramic fuel cell at 1000~ by Baur and Preis in 1937 [1.6]. Nernst discovered solid oxygen-ion conductors when he invented the socalled glower in the end of the 19th century [1.5]. Nernst proposed to use solid compositions such as ZrO2 with 15 wt% Y203 addition (called the Nernst mass) as a glower to replace carbon filaments in electric lamps. The Nernst glower was operated for hundreds of hours on direct current, though electrolysis was found to occur. It was explained that any loss of oxygen liberated at the anode was balanced by an equal amount of oxygen taken into the glower at the cathode. This phenomenon was the reverse of fuel cell operation. In 1935, Schottky published a paper suggesting that the Nernst mass could be used as a fuel cell solid electrolyte [1.7]. In 1937 Baur and Preis demonstrated the operation of the first ceramic fuel cells [1.6]. They used mainly ZrO2-based ionic conductors (e.g., ZrO2 with 10 wt % MgO or 15 wt % Y203 addition) in the form of a tubular crucible as the electrolyte, with iron or carbon as the anode and Fe304 as the cathode. Observed open-circuit voltages were between 1.1 and 1.2 V at 1000 ~ to 1050~ Baur and
TABLE 1.2 Typical Features and Operational Characteristics of SOFC and Other Types of Fuel Cells -
--
-
--
-
-
Type of fuel cell Molten carbonate
Phosphoric acid
Alkaline
Polymer membrane
Solid Y20,-stabilized zrOz (YSZ)
Molten Li,CO,-
H,PO,
KOH solution
Perfluorosulfonic acid membrane
Electrolyte support
None
LiAlO,
Sic
Asbestos
None
Cathode
Sr-doped LaMnO,
Li-doped NiO
PTFE'-bonded Pt on C
Pt-Au
PTFE-bonded Pt on C
Anode
NiIYSZ
Ni
PTFE-bonded Pt on C
Pt-Pd
PTFE-bonded Pt on C
Interconnect/Bipolar
Doped LaCrO,
SS" clad with Ni
Glassy carbon
Ni
Graphite
Operating temperature
1000°C
650°C
200°C
100°C
80°C
Operating pressure
1 atm"'
1 to 3 arm
1 to 8 arm
1 to 10 atm
1 to 5 atm
Fuel
H,. CO
Hz, CO
H?
Hz
H2
Oxidant
0 2
O? + CO,
0,
0,
0,
Contaminant tolerance
< 10-100 ppm sulfur
< ppm sulfur
< lt02%CO < 50 ppm sulfur
No C02, CO No sulfur
< 50 ppm CO No sulfur
Electrolyte
K2C03
11
'PTFE = Polytetrafluoroethylene; "SS = stainless steel; "'atm = 1.01 x 1@ Pa
Introduction
Solid oxide
12
Chapter 1
Preis constructed a ceramic fuel cell battery consisting of eight ZrO2-Y203 crucibles filled with coke and immersed in a common magnetite bath. With hydrogen, CO, or town gas as fuel, the open-circuit voltage was 0.8 V per cell (0.2 V lower than the theoretical value). At a current density of approximately 0.3 mA/cm 2, the cell voltage was 0.65 V, corresponding to an imernal resistance of 1.8 to 2.6 ~. Although operation was demonstrated, the current outputs of these cells were too low to be practical. Initial development work on practical ceramic fuel cells began in the early 1960s. The cell configuration in this time period was either a flat-plate design using the electrolyte in the form of a disk, or a segmented-cell-in-series design (bell-and-spigot configuration) using short tubular segments of the electrolyte joined together with conducting seals. These designs used very thick electrolytes, thus suffering significant internal resistance losses. This led to the development of the thin-wall concept to improve cell performance. In 1970s the banded configuration (a segmented-cell-in-series design) was proposed, which made use of the thin-wall concept in which a number of thin-film cells were deposited on a porous support. Development of fuel cells based on this configuration is still going on; kilowatt-size stacks of banded SOFC cells have been tested. In 1980 the sealless tubular design was proposed, with several advantages over the segmented-cell-in-series design. The key features of the sealless tubular design include individual thin cells formed on a tubular support and electrically connected into a bundle in a fuel-reducing atmosphere. This design is presently the most advanced; multikilowatt sealless tubular SOFC generators have been fabricated and operated for thousands of hours. In 1982 the monolithic design, in which cells are configured in a honeycomb structure (resulting in extraordinarily high power density), was advanced. At the same time, interest in the fiat-plate design has been renewed, and due to many advances in ceramic forming and processing technologies, various advanced fiatplate concepts have been proposed. Early SOFC stacks used noble metals (e.g., platinum) as electrode and interconnect materials. In the early 1970s nickel/YSZ, doped In203, and CoCr204 were used as anode, cathode, and interconnect, respectively. CoCr204 was later replaced by LaCrO3, and in 1980 LaMnO3 and LaCoO 3 were proposed for cathode use. Recently, high-temperature alloys have been tested as interconnect material for flat-plate SOFCs. Figure 1.6 summarizes key historical events in the development of the SOFC technology.
ADVANCED FLAT-PUTE SOFC I
MONOLITHIC SOFC
I
I
SEALLESS TUBULAR SOFC
I SEGMENTED-CELL-IN-SERIES SOFC (BANDED CONFl URATION)
I
'1
I
SEGMENTED-CELL-IN-SERIES SOFC [BELL-AND-SPIGOT)
I
I
CELL OPERATION DISCOVERY OF SOLID ELECTROLYTE
I
I
I
I Introduction
I
IBAUR AND PREIS)
FLAT-PLATE SOFC
YSZ ELECTROLYTE INTERCONNECT Ni/YSZ ANODE In,O, CATHODE CoCr,O, INTERCONNECT
'
I
LaCrO, INTERCONNECT I
b M n O , CATHODE LaCoO, CATHODE
t METALLIC INTERCONNECT
Figure 1.6. Key historical events in SOFC technology development 13
14
Chapter 1
References 1.1
1.2 1.3
1.4 1.5 1.6 1.7
Morgantown Energy Technology Center, Fuel Cells -- Technology Status Report, Report No. DOE/METC-87/0257, Morgantown Energy Technology Center, Morgantown, WV, 1986. N.Q. Minh, J. Am. Ceram. Soc., 76 (1993) 563. N.Q. Minh, in Science and Technology of Zirconia V, S.P.S. Badwal, M.J. Bannister, and R.H.J. Hannink (eds.), Technomic Publishing Company, Lancaster, PA, 1993, p. 652. W.R. Grove, Philos. Mag., 14 (1839) 127. W. Nernst, Z. Elektrochem., 6 (1899) 41. E. Baur and H. Preis, Z. Elektrochem.,43 (1937) 727. W. Schottky, Wiss. VerOff. Siemens Werken, 14 (1935) 1.
Chapter 2 PRINCIPLES OF OPERATION 2.1 GENERAL A solid oxide fuel cell (SOFC) is a ceramic device that converts the chemical energy of a fuel gas and an oxidant gas directly to electrical energy without combustion as an intermediate step. The operating principles of a SOFC and other types of fuel cells are similar to those of a battery, i.e., electrochemical combination of reactants to generate electricity. However, unlike a battery, a SOFC does not run down or require recharging; the fuel cell employs gases (from an external source) as reactants, and operates as long as both fuel and oxidant are supplied to the electrodes. In fuel cells, the electricity generation mechanism is based on the electrochemical combustion of the fuel; i.e., the overall reaction is the same as that of the combustion; however, the reaction is made of two separate electrochemical reactions. For example, for hydrogen fuel and oxygen oxidant, the electrochemical combustion reaction consists of the oxidation of hydrogen at the anode and the reduction of oxygen at the cathode. The overall reaction in this case, like combustion, yields water as the reaction product. In the operation of a SOFC, fuel (e.g., hydrogen) is fed to the anode, where it is oxidized and electrons are released to the external (outer) circuit. Oxidant (e.g., oxygen) is fed to the cathode, where it is reduced and electrons are accepted from the external circuit. The electron flow (from the anode to the cathode) through the external circuit produces direct-current (DC) electricity. The electrochemical transformation of the fuel and oxidant in a SOFC is isothermal; i.e., the fuel cell directly uses the available free energy in the fuel at the operating temperature. Direct conversion of fuel energy to electricity is the key characteristic of fuel cell operation. In a conventional thermal power system, the chemical energy of the fuel is transformed first to thermal energy, then to mechanical energy, and finally to electrical energy. Other' energy systems such as magnetohydrodynamic (MHD) generators and thermionic converters involve the conversion of chemical
16
Chapter 2
energy to thermal energy and then to electricity. The efficiency of the thermalto-mechanical and thermal-to-electrical energy conversions is subject to the Carnot limitation. The Carnot efficiency of a combustion-type system operated between high-temperature (Th) and low-temperature (T/) heat sources is given as e = 1
(Eq. 2.1)
Tt
where e is the efficiency and T is the temperature in K. To obtain a high value of E, a T h as high as possible and a TI as low as possible are desirable. However, there is a practical limit on this efficiency due to high limits on Th (temperature of material stability) and low limits on ~ (room temperature). The operation of a fuel cell is not Carnot-limited. A fuel cell converts chemical energy directly to electricity and thus can yield a higher efficiency than a combustion-type conversion system. For practical power generation applications, a SOFC must use commercially available fuels and produce alternate-current (AC) electricity. Therefore, besides the fuel cell power section, a SOFC system has two other main components: a fuel processor and a power conditioner. The fuel processor converts a practical fuel to a suitable gas that is then fed to the fuel cell stack. The power conditioner uses solid-state technology to efficiently convert DC electricity to AC.
2.2 THERMODYNAMIC PRINCIPLES The operation of a SOFC involves the reduction of the oxidant at the cathode and the oxidation of the fuel at the anode. At present, the most common fuel and oxidant for use in SOFCs are hydrogen and oxygen (electrochemically active). Thus, for SOFCs having an oxygen-ion-conducting electrolyte, the reactions in the fuel cell involve the oxidation and reduction of oxygen at the electrodes. Similarly, for SOFCs having a proton-conducting electrolyte, the reactions involve the oxidation and reduction of hydrogen. At the cathode, the reduction of oxygen in a SOFC based on an oxygenion-conducting electrolyte is given as
O2(c) + 4e-
2-
= 20(e )
(Eq. 2 2)
17
Principles of Operation
where the subscripts (c) and (e) represent the states at the cathode and in the electrolyte, respectively. At the anode, the reverse reaction of Eq. 2.2 can be regarded thermodynamically as the primary electromotive reaction, i.e., (Eq. 2.3)
2-
20(~) = 02(a) -I- 4e-
where the subscript (a) represents the state at the anode. Consequently, the overall cell reaction (which determines cell voltage) is represented by the following equation: O2(c) :
(Eq. 2.4)
O2(a)
The SOFC is therefore considered to be an oxygen concentration cell, and the electromotive force (emf) or reversible (thermodynamic) voltage, Er, is given by the Nernst equation P E, -
R T ln
4F
(Eq. 2.5)
o~)
P o2(a)
where R is the gas constant, T the temperature, F the Faraday, and P o 2 the partial pressure of oxygen at the electrode. For a certain oxygen partial pressure at the cathode, the magnitude of Er depends on the anode oxygen partial pressure, thus on the type and composition of the fuel fed to the anode. For example, when CO is fed to the anode, the following reaction takes place at the anode: (Eq. 2.6)
CO(a ) + 1/~ O2(a ) -- CO2(a)
The oxygen partial pressure at the anode is given by
Po2(a) 9
(Eq. 2.7)
PCO(a)K(2.6)
where K(2.6 ) is the equilibrium constant of Eq. 2.6. Substituting the equation for the anode oxygen partial pressure (Eq. 2.7) into Eq. 2.5 yields RT Er = E0 + ~
4F
LrlPo2~c) +
RT 2F
In
gco(a) Pc02
(Eq. 2.8)
18
Chapter 2
where E ~ is the reversible voltage at the standard state and is given as EO - R T
2F INK(26)
(Eq. 2.9)
Thus, Eq. 2.8 gives the reversible voltage of the cell CO2(a) ,
CO(a)I Oxygen-ion conductor [ O2(c)
(Eq. 2.10)
with the following cell reaction
2CO(a )
-+- O2(c) =
2CO2(a)
(Eq. 2.11)
Similar equations can be obtained when other gases are used as the fuel in the anode. For example, for hydrogen fuel, the cell reaction is
H2(a) d- 1/~O2(c)= H20(a )
(Eq. 2.12)
The reversible cell voltage is given as RT RT PI'I2(a) E~ = E ~ + lnP%,) + - - l n ~ , 4F 2F P~o
(Eq. 2.13)
where E ~ is the standard cell voltage. At the standard state, Er equals E ~ and the following equation is established for every fuel: EO -
AG O zF
AH ~ - T A S ~ zF
(Eq. 2.14)
where AG Ois the standard Gibbs free energy change of the combustion reaction of the fuel, AH ~ the standard enthalpy change, AS~ the standard entropy change, and z the number of moles of oxygen required to oxidize one mole of fuel multiplied by four. The maximum energy obtained in this case is given by -AGO, and the ideal thermodynamic efficiency eT is represented by AG~ Table 2.1 lists AG ~ A//~ E ~ and eT for the combustion of several fuels (when the fuel cell reaction products are in gaseous state). (The efficiency is referred to as low heating value (LHV) when the H20 product is in the form of steam and as high heating value (HHV) when the H20 is produced in the liquid state.)
19
Principles of Operation TABLE 2.1
Thermodynamic Data and Thermodynamic Efficiencies for Several Cell Reactions
Reaction
T, K
AG~ kJ
H2 + 1AO2 = H20
1000 1250
-192.5 -178.2
CO + 1AO2 = CO2
1000 1250
-195.4 -173.2
1000
1250 1000 1250
CH 4 + 202
=
C O 2 -Jr-
C + 02 = CO2
2H20
E~ V
cv
-247.3 -249.8
0.997 0.924
0.78 0.71
-283.3 -283.3
1.013 0.898
0.69 0.61
-802.5
-800.4
1.039
1.00
-802.9
-801.2
1.039
1.00
-396.6 -396.6
-396.2 -396.6
1.027 1.027
1.00 1.00
~,
kJ
The effect of temperature and pressure on the reversible voltage of a fuel cell can be analyzed based on changes in the free energy with temperature and pressure. Thus, the following equations can be derived:
OEr (-~)P OEr (--~) r -
AS
(Eq. 2.15)
- zF AV zF
(Eq. 2.16)
where A V is the volume change. For the hydrogen/oxygen reaction, the entropy change is negative; therefore, the reversible or thermodynamic voltage of the fuel cell decreases with increasing temperature. For the same reaction, the volume change is negative; therefore, the reversible voltage increases with increasing pressure. An increase in the operating temperature is beneficial to fuel cell performance because of enhanced mass transfer, increased reaction rate, and usually lower material resistance (thus reduced cell polarization). Increase in operating temperature, on the other hand, may limit material choice and
20
Chapter 2
accelerate material-related problems such as interaction, degradation, and sintering. An increase in the operating pressure improves fuel cell performance because of increased reactant partial pressure and increased mass transport rate. On the other hand, increase in pressure also imposes limits on material selection and causes other problems or concerns such as integrity of the gas seal and cell structure. In reversible operation, the heat absorbed by the fuel cell at constant temperature equals the change in entropy of the reactants Q, = TA S = A H -
AG
(Eq. 2.17)
If the change in entropy is negative, as is the case in most common fuel cell reactions, heat is generated by the cell. In practical fuel cell operation, this heat increases the operating temperature. Performance losses due to higher temperatures are generally avoided by cooling the cell to remove the heat generated. 2.3 FUEL CELL EFFICIENCY The overall efficiency of a SOFC, EFC, is the product of the electrochemical efficiency 6E and the heating value efficiency ell. The electrochemical efficiency is, in turn, the product of the thermodynamic or thermal efficiency er, the voltage efficiency ev, and the Faradaic or current efficiency ej of the fuel cell. Thus, %c = e~ea = exeveJea
(Eq. 2.18)
A fuel cell system consists of, in addition to the fuel cell, the fuel processor and the power conditioner. Thus, the efficiency of a SOFC system without byproduct heat utilization, es, is given as r
=r
e'aveve
(Eq. 2.19)
where EFp and Epc are the efficiencies of the fuel processor and power conditioner, respectively. If the byproduct heat is used in a bottoming cycle and/or for cogeneration, the system efficiency 6s/H is then given by the ratio of the total AC power plus bottoming cycle and cogeneration heat to the high heating value (HHV) of the fuel fed to the fuel processor. The various efficiencies mentioned above are generally independent of each other and can be optimized separately.
Principles of Operation
21
2.3.1 Electrochemical efficiency The electrochemical efficiency of a SOFC includes three elements: the thermodynamic efficiency, the voltage efficiency, and the current efficiency (often referred to as the fuel utilization). (i) Thermodynamic efficiency: In a SOFC and other types of fuel cells, the Gibbs free energy change of the cell reaction may be totally converted to electrical energy. Thus, a fuel cell has an intrinsic (maximum) thermodynamic efficiency given by
AG
er - AH - 1
TAS AH
(Eq. 2.20)
For common fuels such as hydrogen, CO, and hydrocarbons (negative AH and negative AS), the thermodynamic efficiency of a SOFC is < 1. (eT of >_ 1 is conceptually possible for cell reactions with positive AS.) (ii) Voltage efficiency: In an operating SOFC, the cell voltage is always less than the reversible voltage. As the current is drawn from the fuel cell, the cell voltage falls, due to various losses. The reduction in the cell voltage under current load depends on current density and several factors such as temperature, pressure, gas flow rate and composition, and cell material. (This reduction is not characteristic of high-temperature SOFCs, but is common not only to all types of fuel cells but also to all electrochemical cells.) The voltage efficiency, ev, is defined as the ratio of the operating cell voltage under load, E, to the equilibrium cell voltage, Er, and is given as ev -
E
e,
(Eq. 2.21)
(It should be noted that the equilibrium voltage, commonly referred to as the open-circuit voltage, may be different from the reversible voltage if there are side reactions, gas cross leakage, etc.) The difference between the operating cell voltage and the expected reversible voltage is termed polarization, overvoltage, or overpotential and is presented as r/. The total polarization of a cell, r/, is the sum of four types of polarization: charge transfer or activation polarization rlA, diffusion or concentration polarization rio, reaction polarization r/~, and resistance or ohmic polarization r/a: TI = TIA + ~ D + ~ R + ~ O
(Eq. 2.22)
Chapter 2
22
Polarization cannot be eliminated but can be minimized by material modification and cell design. Temperature, pressure, electrolyte composition, and electrode material naturally influence cell polarization. For example, increasing temperature enhances mass transfer, increases the reaction rate, and usually decreases cell resistance, thus reducing cell polarization and increasing voltage efficiency. (a) Charge transfer or activation polarization" Chemical reactions including electrochemical reactions involve an energy barrier that must be overcome by the reacting species. This energy barrier, called the activation energy, results in activation or charge transfer polarization, r/A. The activation polarization may be regarded as the extra potential necessary to reduce the energy barrier of the rate-determining step of the reaction to a value such that the electrode reaction proceeds at a desired rate. Activation polarization is related to current density, j, by the following equation:
J =joexp
RT J - j ~
~-~
(Eq. 2.23)
where a is the transfer coefficient,, and Jo is the exchange current density. The transfer coefficient is considered as the fraction of the change in the polarization which leads to a change in the reaction rate constant. The exchange current density is the (equal) forward and reverse electrode reaction rate at the equilibrium potential. High exchange current density means high electrochemical reaction rate and, thus, good fuel cell performance might be expected. The exchange current density can be determined experimentally by extrapolating plots of log j versus r/to r/ = 0. When the irreversibility of the electrode reaction is small, the second term on the right hand side of Eq. 2.23 may be neglected, and by taking the common logarithms for both sides of Eq. 2.23, the Tafel equation is obtained rlA = a • b logj
(Eq. 2.24)
where a and b are constants which are related to electrode material and type of electrode reaction. Charge transfer or activation polarization is generally due to one or more slow rate-determining steps in the electrode reaction. The slow step could be related to adsorption of reactant onto the surface of the electrode, electron transfer, desorption of product, or any other step in the reaction. The electrode reaction rate is a function of temperature, pressure, and electrode material. At
Principles of Operation
23
high temperatures as in the case of SOFCs, reaction rate is rapid, and as a result, charge transfer or activation polarization is usually small. (b) Diffusion or concentration polarization: Diffusion or concentration polarization, riD, appears when the electrode reaction is hindered by mass transport effects, i.e., when the feeding velocity of the reactant and/or the removing velocity of the reaction product from the electrode is slower than that corresponding to the discharge currentj. When the electrode process is governed completely by diffusion (because of low concentration of reactant in the feed gases or because of reactant conversion approaching 100 %), the limiting current, JL, is reached (characterized by a rapid drop in cell voltage). The limiting current can be calculated from the diffusion coefficient of the reacting ions, D, the activity of the reacting ions, aM~§ and the thickness of the diffusion layer, di, by applying Fick's law as JL -
zFDaMz
+
(Eq. 2 25)
8
For an electrode process free of activation polarization, the diffusion or concentration polarization is expressed as
llD _ R T l n ( I _ j_" ] zF t
(Eq. 2.26)
The diffusion polarization is dependent on the mass transport properties of the system. Mass transport is a function of temperature, pressure, concentration, and the physical properties of the system. In SOFCs, the reactants must diffuse through the porous anode and cathode so the electrode structure is important. Since the electrode reaction rate is a function of the concentration of the reactant gases, the diffusion polarization becomes more severe as the degree of conversion increases. (c) Reaction polarization: The reaction polarization, r/R, appears when the rate of the reaction to supply cell reactants or to remove products (in the vicinity of the electrode before or after the cell reaction) is slow. This polarization is similar to the concentration polarization. At high operating temperatures, the reaction polarization is usually small. (d) Resistance or ohmic polarization: The ohmic polarization is caused by resistance to conduction of ions (through the electrolyte) and electrons (through the electrodes and current collectors), and by contact resistance between
Chapter 2
24
cell components. The ohmic polarization, r/,, is given as
TI~ - jR~
(Eq. 2.27)
where R i represents the total cell resistance, including both ionic and electronic resistances. (The resistance polarization is commonly separated from other types of polarization and referred to as ohmic loss.) (iii) Current efficiency: The efficiency of a SOFC falls if all of the reactants are not converted to reaction products, or if some electrons are involved in an alternative reaction such as corrosion. For 100% conversion of fuel, the amount of current density, j'~, produced is given as (Faraday's law)
Jp
-- zF df dt
(Eq. 2.28)
where f represents the amount of fuel and t the time (df/dt is the molar flow rate of the fuel). For the amount of fuel actually consumed, the current density produced is given by
(If
(Eq. 2.29)
The current efficiency, ej, is the ratio of the actual current produced to the current available from complete electrochemical conversion of the fuel ej
=
J
m
(Eq. 2.30)
In the case of fuel cells, current efficiency is commonly expressed as fuel utilization. Since high utilization of fuel in a fuel cell in general and a SOFC in particular results in increased diffusion polarization, fuel cells are often operated at less than 100 % fuel utilization. 2.3.2 Other efficiencies
In addition to the electrochemical efficiency, other efficiencies considered in a SOFC system are the heating value efficiency and the system efficiency. (i) Heating value efficiency." The heating value efficiency must be considered in cases where the fuel contains inert gases, impurities, and other combustibles in addition to electrochemically active species (hydrogen) [2.1]. In general, gases produced from practical fuel processors contain varying amounts
Principles of Operation
25
of inerts, particles, and combustibles. A heat engine is capable of converting all the chemical energy of combustible materials into heat energy. Some of these may not be utilized in a fuel cell, even at the high operating temperatures of the SOFC. The heating value efficiency, ~,, is defined as the ratio of the amount of heat energy of fuel species available in the fuel cell to generate electricity, AH ~ to the amount of heat energy included in all combustible species in the fuel gases fed to the fuel cell, AHcom (both at the low heating value because water product is generally not condensed in the fuel cell) ea =
AH ~
aH~om
(Eq. 2.31)
This efficiency may be close to unity for high-temperature SOFCs operating on simple fuels such as methane. (ii) System efficiency: As discussed earlier, the fuel cell efficiency (~Fc) considers only the fuel cell power section in a fuel cell system. The efficiency of the system should include the efficiencies of the fuel processor, power conditioner, and byproduct heat utilization. The fuel cell system efficiency, Es/., is expressed as Csm =
Fuel Cell(A C) +Bottoming Cycle(A6")+Cogeneration(Heat) Raw Fuel into FueIProcessor(HHlO
(Eq. 2.32)
In this case, a bottoming cycle is used to generate additional electricity using fuel cell byproduct heat in a gas turbine or steam turbine. Cogeneration uses the fuel cell byproduct heat for space heating, to supply hot water, or to generate steam for industrial process. 2.4 P O W E R G E N E R A T I O N
A typical voltage/current plot of an operating SOFC is presented in Figure 2.1. The figure illustrates the regions in which various types of voltage losses predominate. From Figure 2.1, it can be seen that at low current densities, the major contribution to the cell voltage losses is from the activation polarization, as indicated by the sharp drop in cell voltage with increasing current. As the current increases, the resistance polarization or ohmic loss dominates, as exhibited by the linearity in Figure 2.1. At high current densities, the cell resistance is controlled by mass transport limitations, resulting in a rapid decrease in cell voltage. Under ideal conditions (i.e., all the polarization losses
26
Chapter 2
REVERSIBLECELLVOLTAGE ~--f
VOLTAGELOSSESDUE TO
V o , r ~ E ,oss~s DuE To
OHMIC DROP
\ /,~
.=VOLTAGE .... LOSSESDUE TO O,FFUsloN o VEn~TENTIAL
CELL CURRENT
Figure 2.1. Typical voltage~current relation for an operating fuel cell
are zero), one would expect constant voltage, i.e., a straight line parallel to the current axis, as indicated by the dotted line in Figure 2.1. The power output Pw of a fuel cell is the product of the voltage and current Pw -- E1
(Eq. 2.33)
where I is the current. Qualitatively, one can predict the nature of the power/current relation by examining the behavior at low and high currents. At low currents, I ~ 0, and at high currents, E ~ 0. Hence, the power values approach zero at both ends. A current at which the power is at a maximum lies between these two extremes. Figure 2.2 is a qualitative presentation of the power/current relation in a hypothetical fuel cell. The hypothetical curve, corresponding to no overpotential losses in the fuel cell, is also shown. It should be stressed that the power/current plot in Figure 2.2 refers to ideal single-cell fuel cells in which planar electrodes are used. In most typical fuel cells, owing to the sophisticated construction of the porous gas diffusion electrodes, the limiting current density is not reached, even at high currents, and the cell voltage/current is approximately linear. In such cases, the power/current relation tends to be parabolic. It is difficult to obtain a general expression for maximum power when all forms of overpotential are present. However, this may be done for some limiting cases, e.g., the case where the cell voltage varies linearly with the
27
Principles of Operation
/ IDEALPOWER/CURRENT RELATIONWITHOUT
o
/ /
MAXIMUM .OWE,
POWER SHUTDOWN DUETO MASS TRANSPORT LIMITATION~
/ / Y
//'/
DUETO 0HMIC LOSSEs BETWEENELECTRODES
APOcWECALOoSNEoSvDU S EpoTT~NT,AL CURRENT
Figure 2.2. Typical power~current relation for a hypothetical fuel cell
current. In this case, the equation for the cell voltage as a function of current is given by E = E , . - Rt/ where
Rt
(Eq. 2.34)
represents the total polarization loss (essentially ohmic loss). Hence, Pw = I(E~ - Rtl)
(Eq. 2.35)
Eq. 2.35 shows that the power/current variation is parabolic. The conditions for the maximum power can be deduced as I -
E
~ 2R t
(Eq. 2.36)
e - Er
(Eq. 2.37)
2 Then, the maximum power is given as P
_ E~ w(m~x)
(Eq. 2.38)
4R t
Thus, the maximum power is realized when the cell voltage is equal to one-half the reversible voltage. At maximum power, voltage efficiency is 50%.
Chapter 2
28
2.5 CHARACTERISTICS OF CERAMIC FUEL CELLS
Compared with the other types of fuel cells, ceramic fuel cells, or SOFCs, characteristically have all-solid-state construction (mainly ceramic), along with high operating temperatures (highest among the present generation of fuel cells). These two characteristics give rise to a number of distinctive features in the SOFC. For example, because all the cell components are solid, the SOFC can be configured into compact and lightweight structures unachievable in fuel cell systems having a liquid electrolyte. In addition, the SOFC uniquely has the characteristic of the possibility of mixed (ionic and electronic) conduction in the solid oxide electrolyte. The presence of electronic conduction in the electrolyte can significantly influence fuel cell efficiency. 2.5.1 Features
Solid oxide fuel cells (and other types of fuel cells) offer several advantages over conventional methods of power generation: higher conversion efficiency, modular construction, high efficiency at partial loads, minimal siting restrictions, and production of far fewer pollutants. As compared with the other types of fuel cell, SOFCs exhibit the following features [2.2]: (i) At the high operating temperatures of the SOFC, electrode reactions are rapid; therefore, catalysts are not needed for the electrodes. On the other hand, because of these high operating temperatures, material selection is limited and material compatibility can be a serious problem. (ii) SOFCs do not suffer from CO poisoning. In fact, CO can be used directly as fuel in SOFCs. The SOFC can tolerate a relatively high impurity content in the fuel. (iii) SOFCs have multifuel capability. In addition to hydrogen, suitable fuels include gasoline, alcohol, natural gas, synthetic gas made from coal or plant matter, and a number of other possibilities. Because of the high operating temperatures, hydrocarbon fuels can be reformed internally within the fuel cell. Thus, expensive external fuel reforming equipment is not necessary. (iv) The SOFC produces useful high-temperature, quality heat suitable for use in cogeneration or bottoming cycles. The overall efficiency of the system can be significantly increased when this byproduct heat is fully utilized.
Principles of Operation
29
(v) Because the SOFC electrolyte is solid, electrolyte management (to prevent electrolyte loss and composition change) is not a problem. Unlike fuel cell systems having a liquid electrolyte, SOFCs need not store excess electrolyte. (vi) Because of its all-solid state, the SOFC can be configured into geometries impossible in fuel cells having a liquid electrolyte. However, fabrication of SOFC cell components into the required structure is often a technical challenge. (vii) SOFC components exhibit relatively low electrical conductivity. Fabricated cell components must be very thin to reduce internal resistance losses. 2.5.2 Effect of electronic conduction in electrolyte In SOFCs, the electrolyte is an ionic oxide. Because the electrolyte is an ionic solid, its electronic conductivity cannot be absolutely zero (see Chapter 3). In general, the SOFC electrolyte is selected such that the electronic transference number is as small as possible under normal operating conditions to minimize electronic conduction losses. However, in some cases, depending on the partial pressure of oxygen at the electrodes, the electronic conduction in the electrolyte cannot be neglected. Even if an electrolyte having some electronic conduction is used, a higher-efficiency output may possibly be obtained if the absolute value of the ionic conductivity of the mixed conducting electrolyte is higher than that of a purely ionic conducting electrolyte [2.3]. When a SOFC is constructed with a mixed oxygen-ion and electronic conductor, the electronic current flows through the electrolyte even at opencircuit conditions. In this case, the terminal voltage, E/, is somewhat lower than the theoretical voltage of the cell reaction, E. The transference number of the oxygen ion, ti, is given as t~ -
'
(Eq. 2.39)
where tyi is the oxygen-ion conductivity and a is the total conductivity (the sum of the oxygen-ion conductivity ai and the electronic conductivity ae). Under this condition, the equivalent circuit of the ceramic fuel cell in operation can be represented as shown in Figure 2.3. The cell can be considered to be short circuited by the resistor, the resistance of which is L/a e where L is the thickness of the electrolyte.
30
Chapter 2
CELL
CATHODE
ANODE I =
I I
=p--
1 I ,--1--. I I
I
I
L
m
.
.
.
.
I
,..,,,
._J
E/
J J
OUTER CIRCUIT
Figure 2.3. Equivalent circuit of an operating SOFC [2.3]
Thus, E / = je L-~- = E - ji L II e
(Eq. 2.40)
O i
where j~ and Ji represent the electronic and ionic current density in the electrolyte, respectively. At the open circuit of the cell, (Eq. 2.41)
j , = j~
The following equation is established: g/ =
Eo.
'
(Eq. 2.42)
O e+ff i
When the cell is discharged through the external circuit, the electronic current in the electrolyte decreases as the terminal voltage of the cell falls. The following equation can be derived for j~: Je = (1 - ti) ( o Et i - J)
(Eq. 2.43)
where j is the current density output, which is given by Ji -J~. The total energy generated by the fuel cell reaction consists of the Joule heat due to Ji (Pw(i)) and j~ (Pw(e)) and the power output Pw. These quantities can
Principles of Operation
31
be represented by the following"
Pw(i) = ( E -
(Eq. 2.44)
E/)ji
Pw(,) = E(i, Pw = E(] = t~Ej
(Eq. 2.45)
j2
(Eq. 2.46)
12
From these equations, the total power, Pw~o), is
Pw(o) = Pw(o + Pw(~) + Pw = E(j + j~)
(Eq. 2.47)
The energy efficiency, e, of the cell is the ratio of power output to total power e -
P
w Pw(o)
(Eq. 2.48)
Then, the relation between energy efficiency and current output is expressed by the following equation:
oEti j _ j2
e =
(Eq. 2.49)
oE[ti(1 - ti)oE + tiJ ] Figure 2.4 shows the relation between e and j, for constants E and o, with ti as a parameter. From this figure, it is evident that the efficiency of the cell with 1,0
I O.B
m z 0.6
u
!!1
0.4
0.2
0.0,
0.0
0.2
0.4 0.6 o.e CURRENT OUTPUT, aE
--i .0
Figure 2.4. Relation between energy efficiency and current output for a constant total conductivity [2.3]
32
Chapter 2
a mixed-conducting electrolyte is lower than that of the cell with a purely ionic conductor in the whole range of current output (for a constant value of total conductivity). However, if the total conductivity of the mixed-conducting electrolyte is greater than that of the purely ionic conductor, the efficiency of the cell may be greater than that of a cell with a purely ionic conductor above a certain current output (Figure 2.5). Under the conditions in Figure 2.4, the current providing maximum energy efficiency can be calculated from O~/aj = 0 and is given as
Je==
=
- (1-ti)]
~
(Eq. 2.50)
Substituting Eq. 2.50 for j in Eq. 2.49, the maximum energy efficiency, 6max, can be obtained as e=~x =
1-~/(1-ti)
(Eq. 2.51)
1 +~/(1-ti) As can be seen from Eq. 2.51, the maximum energy efficiency is dependent only on the oxygen-ion transference number and is independent of total conductivity and theoretical emf. This is an important criterion for the selection of solid oxygen-ion conductors for SOFC electrolytes. The relationship between 6max and ti is shown in Figure 2.6. 1.0
0.8
U 0.6
I-////
E
.~eo. 0.4
e
,,z
"%.
~o
0.2 |l/
o or 0.0
'='6,~
0.2
,
0.4
0.6
%,
L0.8- %
1.0
i.
CURRENT OUTPUT, aoE
Figure 2.5. Relation between energy efficiency and current output for various conductivities [2.3]
33
Principles of Operation
1.0
0.8
0.6
0.4
0.2
I 0.0
0.0
0.2
1
I
I
0.4
0.6
0.8
1.0
TRANSFERENCE NUMBER OF OXYGEN ION
Figure 2.6. Relation between maximum energy efficiency and oxygen-ion transference number [2.3]
The power output at maximum energy efficiency can be obtained as
Pw(emx,=oE2/(l_ti)[l_/(l_ti)~
(Eq. 2.52)
This equation is shown graphically in Figure 2.7, indicating that a maximum value of Pw~, max) is obtained at ti = 8/9. The relation between the power output and the energy efficiency is an important consideration in designing the construction of the ceramic fuel cell. This relation can be derived by eliminating j from Eqs. 2.46 and 2.49 and is given as
Pw = loE2eti{[(1-e)zt~-4r 2
As
ti --" 1, Pw approaches
(1-r
(l-Q}
(Eq. 2.53)
the following formula:
Pw
= ~162 1 - e)
(Eq. 2.54)
The relation between Pvr and E for various values of ti, with constants E and a, is shown in Figure 2.8. In these curves, the arrows show the direction of the increase in current output. The power output at maximum energy efficiency does not coincide with the maximum power output. Figure 2.8 shows that higher power output can be
34
Chapter 2
0.15 tu tO LL 14. ILl
0.10 X II--
0.05
I0 re. l,iJ
O.OO 0.0
0
I
!
1
1
0.2
0.4
0.6
0.8
TRANSFERENCE
NUMBER
1.0
OF OXYGEN
ION
Figure 2.7. Relation between power output at maximum energy efficiency and oxygen-ion transference number [2.3]
0.25
0.20
O.15
,,=,
"o
0.10
0.05
0.00 i . 0.0
4
I
0.2
0.4
0.6
0.8
1.0
E N E R G Y EFFICIENCY
Figure 2.8. Relation between power output and energy efficiency for various oxygen-ion transference numbers [2.3]
obtained for a slight loss of efficiency (since the slope of the Pw-versus-e curve is very steep in the vicinity of maximum efficiency). As shown in Eq. 2.53, the power output of the cell is a complicated function of e and ti, but proportional to tr. For the purpose of discussing the relation among these four quantities, it is convenient to add a a-Pw relation to Figure 2.8 (Figure 2.9). Using Figure 2.9, the characteristics of various cells
Principles of Operation
.
.
.
.
3=3
"u 0
.
O
"
~
\
IX / i \ !
I
g
0.10 zo E7 C 0
0.6
!
1
0.5
0.4
! I 0.31
, 0.2
0.1
0.0
POWER OUTPUT (TOTAL CONDUCTIVITY o'), o'k..=
0.2
_o.oo r 0.4
I 0.6,
0.8
1.0
o~j
ENERGY EFFICIENCY
Figure 2.9. Relation between energy efficiency and power output with respect to conductivity and oxygen-ion transference number [2.3]
can be compared with respect to their energy efficiencies and power outputs, if the conductivities and oxygen-ion transference numbers are known. For example, consider two cells, I and II, the electrolytes of which have total conductivities of a/and a~/(a/ < %) and oxygen-ion transference numbers of ti,~ and ti,~/(ti,~ > ti, z/), respectively. When cells I and II are operated in the vicinity of ~ = ~K, cell II has a higher output power than cell I. In this case, the cell having the electrolyte with the smaller oxygen-ion transference number shows the higher output. In the vicinity of ~ = ~L (EL > EK), however, the power output of cell I is superior to that of cell II. Table 2.2 lists the ratio of total conductivity of the mixed conducting electrolyte to that of a purely ionic electrolyte giving the same efficiency. For example, in order to get an efficiency of 0.60 using an electrolyte with the oxygen-ion transference number of 0.94, the conductivity of the electrolyte needs to be 1.5 times that of the purely ionic conductor.
Chapter 2
36
TABLE 2.2 Ratio of Total Conductivity of Mixed-Conducting Electrolyte to That of Purely Ionic Electrolyte for Various Values of t i and e [2.3]
Efficiency 0.35 0.40 0.45 0.50 0.55 0.60 0.65 0.70 0.75 0.80 0.85
1.000
1.0
1.0
1.0
1.0
1.0
0.995 0.990 0.980 0.960 0.940 0.920 0.900 0.850 0.800
1.1 1.1 1.1 1.1 1.1 1.2 1.2 1.3 1.6
1.1 1.1 1.1 1.1 1.2 1.2 1.2 1.4
1.1 1.1 1.1 1.1 1.2 1.2 1.3
1.1 1.1 1.1 1.1 1.2 1.3 1.4
1.1 1.1 1.1 1.2 1.3 1.5
1.0 1.1 1.1 1.1 1.2 1.5
1.0 1.1 1.1 1.2 1.5
1.0
1.0
1.0
1.1 1.1
1.1 1.2
1.1 1.4
1.3
1.5
1.0 1.5
It is clear from Eq. 2.54 that an oxygen-ion transference number of greater than 0.89 is necessary to yield an energy efficiency greater than 0.5. Therefore, for SOFCs, the oxygen-ion transference number in the electrolyte must be greater than 0.9. However, it is clear that, even if the electrolyte shows some electronic conduction, the cell can give high power with fairly high efficiency when its oxygen-ion transference number is not smaller than 0.9, provided that its conductivity is sufficiently high. 2.6 TYPES OF FUEL AND OXIDANT In theory, any gases capable of being electrochemically oxidized and reduced at the fuel cell operating temperature can be used as fuel and oxidant. However, hydrogen is currently the most common fuel, and oxygen the most common oxidant for use in SOFCs.
Hydrogen can be derived from many
practical fuels such as natural gas, alcohol, or coal. Oxygen is readily available from air.
Principles of Operation
37
2.6.1 Fuel
Present ceramic fuel cells use exclusively hydrogen as the fuel. Hydrogen can be obtained from a number of hydrogen-containing fuels, e.g., natural gas, or from synthesis gases obtained by gasification of carbon sources, e.g., coal. Among the practical fuels for the SOFC, hydrocarbons are probably the most common. Hydrocarbon fuels are thermodynamically unstable at the high operating temperatures of the SOFC. For example, pipeline natural gas (which consists primarily of methane with small quantities of the higher hydrocarbon gases such as ethane and propane, and trace amounts of a sulfurbearing odorant such as mercaptan, aliphatic sulfides, and thiophene) decomposes mainly into carbon and hydrogen at fuel cell operating temperatures. An appropriate amount of steam is often added to prevent carbon deposition and to reform the hydrocarbons. The steam reforming of hydrocarbons can be carried out in an external reformer (external reforming) or within the fuel cell (internal reforming). Sulfur impurities, often present in common fuels, tend to cause cell performance to degrade and to retard or poison the reforming activity of cell materials even when steam is added to the fuel. Therefore, if undesirably high levels of sulfur are present, the fuel must be desulfurized before fed to the fuel cell. One common fuel for use in SOFCs is natural gas. The thermodynamic feasibility of reforming natural gas in the SOFC depends on sufficient heat being available at a suitable temperature for the endothermic reforming reaction. In general, the electrochemical reactions produce enough heat for use in internal reforming. For example, in the case of methane, the heat produced by the electrochemical oxidation reaction at the SOFC operating temperature is about twice that required by the reforming reaction. Potential liquid fuels for SOFCs are naphtha, gas oil, or kerosene. In this case, external reformers are often required. Also, sulfur must be removed from the fuel before steam reforming. In general, the heavier the liquid fuels, the higher the sulfur content, and the more difficult the fuel is to desulfurize. Alcohol can also be used as the fuel; it can be reformed internally to supply hydrogen for the SOFC. Another potential source of fuel for the SOFC is coal. Coal may be gasified externally through steam/carbon reaction to produce hydrogen and carbon monoxide for SOFCs. Usually, coal is reacted with steam and oxidant (air or oxygen) in a pressurized, fluidized-bed gasifier to produce hot synthesis
Chapter 2
38
gas. Coal can also react with hot CO2 and H20 (which are the products from ceramic fuel cells) to form hydrogen and CO. The heat produced by the fuel cell can be used to sustain the gasification process [2.4,2.5]. Biogas and gases from biomass and landfill wastes are also potential fuel gases for ceramic fuel cells. The composition of such gases is determined by its respective origin and its generation process [2.6]. For example, gas mixtures produced by anaerobic digestion of manure are rich in methane and contain a certain amount of sulfur and a small amount of halides. Landfill gases have the composition similar to that of a biogas; however, they contain ammonia, some chlorides, and carbon-fluorine compounds. Biomass can be gasified either by high-temperature pyrolysis [2.7,2.8] or by partial oxidation [2.9]. Sulfur removal is usually necessary for biogases [2.10] but direct utilization of biogases in the fuel cell is possible when contaminants do not exceed a certain limit
[2.11]. 2.6.2 Oxidant
The performance Of ceramic fuel cells is improved when pure oxygen is used as the oxidant; however, air is usually used because of its availability. The difference between cell voltage obtained with pure oxygen and that with air increases as the current density increases, suggesting that diffusion polarization plays an important role during the reduction of oxygen in air. Because of the high operating temperature, a SOFC system needs an air supply blower, air preheater, and air recirculator. 2.7 FUEL-PROCESSING SYSTEM The function of a fuel-processing system is to convert practical fuels to a gas mixture suitable for use in the fuel cell. For natural gas and liquid fuels, the fuel processor consists mainly of sulfur removal and reforming systems. For coal, the fuel-processing system consists of gasification, cleanup, and desulfurization subsystems. The fuel-processing system for natural gas is often designed to remove sulfur compounds to below 0.1 ppm, using active carbon, zinc oxide, or hydrogen (hydrodesulfurization). The desulfurization method selected depends on the sulfur compounds involved. For example, when the fuel contains thiophane, a hydrodesulfurization reactor is usually installed in the fuel-
Principles of Operation
39
processing system in series before the zinc oxide reactor. After desulfurization, natural gas is reformed, either externally or internally. For internal reforming, natural gas is fed to a prereformer before being reformed within the boundaries of the SOFC (reforming partially in prereformer tubes and partially in the fuel cell), or is reformed within the cell without a prereformer (100% reforming in the fuel cell). In both cases, a portion of the spent f,,el stream is recirculated, to guarantee a supply of water vapor adequate to support the reforming reaction. For heavier liquid fuels, because of difficulties in sulfur removal and cost concerns, reformers need high sulfur tolerance. This requires higher operating temperatures for the reformer and/or the use of reforming catalysts that have less overall reforming activity but are also less sensitive to sulfur poisoning. Heavier liquid fuels also contain higher proportions of aromatic hydrocarbons. This leads to another severe technical p r o b l e m - carbon formation in the reformer. These two factors, sulfur tolerance and carbon formation, have been the key challenges in the development of fuel processors for heavy hydrocarbon liquid fuels. For the conversion of heavier liquid fuels, high-temperature steam reforming, autothermal reforming, hybrid reforming, and cyclic reforming have been considered
[2.12]. For coal, a pressurized, fluidized-bed gasifier (aair- or oxygen-blown) is used to produce coal gases. Carbon conversion reaches 98.5 %, and examples of gas compositions produced (in vol %) [2.13] are
H2
CO
CH 4
H20
CO2
N2
H2S
COS
NH 3
Air mode
16.8
27.9
1.8
3.8
2.8
46.0
0.68
0.02
0.16
Oxygen mode
29.4
38.0
4.0
17.3
9.5
0.54
1.07
0.02
0.24
The gas from the gasifier is cooled in a steam generator after removal of entrained particulates. The cooled gas is treated in order to remove sulfur compounds by absorption on beds of zinc ferrite or zinc oxide. The clean gas is then passed through an expander before it flows into the fuel cell.
2.8 POWER-CONDITIONING SYSTEM A fuel cell produces DC currem at a certain voltage. If the DC current is used directly (e.g., supply power to an electrolyzer), a chopper is required for controlling the voltage output. For other applications, a power-conditioning system is required in order to convert the DC current to an AC current consistent with, for example, the electric utility interface standards. A power-conditioning
Chapter 2
40
system may have a self-commutated inverter or an externally commutated inverter for commutation of DC to AC, and a self-controlled inverter or an externally controlled inverter for frequency control.
For a fuel cell power-
conditioning system, the self-commutated inverter is commonly used.
When
connecting to a commercial AC line system, the self-controlled inverter is used, and in the case of a simple AC system, the externally controlled inverter is often used.
References 2.1 2.2
2.3 2.4 2.5
2.6
2.7 2.8 2.9 2.10
2.11 2.12
2.13
E.H. Camara and L.G. Marianowski, Handbook of Fuel Cell Performance, Institute of Gas Technology, Chicago, IL, 1980, p. 83. J.L. Bates, in Proceedings of the 16th Energy Technology Conference, February 28March 2, 1989, Washington, DC, Government Institutes, Rockville, MD, 1989, p. 205. T. Takahashi, K. Ito, and H. Iwahara, Electrochim. Acta, 12 (1967) 21. R.L. Zahradnik, L. Elikan, and D.H. Archer, in Advances in Chemistry Series 47, Fuel Cell Systems, American Chemical Society, Washington, DC, 1965, p. 343. Westinghouse Electric, 1970 Final Report Project Fuel Cell, Research and Development Report No. 57, U.S. Government Printing Office, Washington, DC, 1970. H. Wendt, V. Plzak, and B. Rohland, in Proceedings of the Second International Symposium on Solid Oxide Fuel Cells, July 2-5, 1991, Athens, Greece, F. Grosz, P. Zegers, S.C. Singhal, and O. Yamamoto (eds.), Commission of the European Communities, Luxembourg, 1991, p. 343. W. Kaminsky, Chem.-Ing. Tech., 61 (1989) 775. D.S. Scott, J. Piskorz, M.A. Bergougnou, R. Graham, and R.P. Overend, Ind. Eng. Chem. Res., 27 (1988) 8. W. Adlhoch and N. Briingel, Braunkohle, 41 (1989) 42. E. Pilarczyk and K. Knoblauch, in Proceedings of the Engineering Foundation Conference on Separation Technology, April 27-May 1, 1987, Elmau, Germany, Engineering Foundation, New York, 1987, p. 522. H.H. M6bius and B. Rohland, U.S. Patent No. 3402078, 1964. J.E. Young, in Proceedings of the Symposium on Fuel Cells: Technology Status and Applications, November 16-18, 1981, Chicago, IL, Institute of Gas Technology, Chicago, IL, 1982, p. 153. M. Krumpelt, V. Minkov, J.P. Ackerman, and R.D. Pierce, Fuel Cell Power Plant Designs: A Review, Report No. ANL-85-39, Argonne National Laboratory, Argonne, IL, 1985, p. 31.
Chapter 3 ELECTRICAL CONDUCTION IN CERAMICS 3.1 GENERAL The operation of a SOFC is based fundamentally on electrical conduction in the ceramic components. The electrolyte conducts ions between the anode and cathode. The electrodes carry electrons to and from the reactive sites, where the electrochemical reactions take place. The interconnect conducts electrons from the anode of one cell to the cathode of the next in electrical series. Thus, electrical conduction processes in ceramics in general and SOFC materials in particular are of paramount importance to the operation of the SOFC. A discussion of electrical conduction in ceramics is given here to provide a background on the basic electrical processes in fuel cell operation. Emphasis is placed on the discussion of electrical conduction in fluorite-type oxides and perovskite oxides, the two common types of oxide used in SOFCs. In general, electrical conduction in ceramics or crystalline solids depends on the material lattice defects. Lattice defects can be classified into two groups: (i) stoichiometric defects, in which the crystal composition is unchanged when defects are formed in the lattice and (ii) nonstoichiometric defects, which are formed as a consequence of a change in the crystal composition. For example, AgC1 crystals may contain Ag + ion interstitials (silver ions in interstitial sites) and Ag + ion vacancies (missing silver ions from their normal sites), thus having stoichiometric defects. Y203-stabilized ZrO2, strontium-doped LaMnO3, and doped LaCrO3 (commonly used as SOFC electrolyte, cathode, and interconnect, respectively) are doped crystalline oxides, thus having nonstoichiometric defects. Alternatively, defects can be classified into three groups by the size and shape of the defect: (i) point defects which involve interstitials or vacancies, (ii) line defects (dislocations) which are effectively point defects in two dimensions, and (iii) plane defects, in which the whole layer in a crystal structure is defective. Although the concept of isolated point defects has become less attractive in recent years (being replaced by microdomain and cluster models),
42
Chapter 3
it is convenient to discuss (and easy to understand) electrical conduction in crystalline oxide ceramics in terms of the three classical types of point defect. These three classical types are the Frenkel defect and the Schottky defect (intrinsic point defects), and the Koch-Wagner defect (extrinsic point defect). The Frenkel-type defect was introduced by Frenkel in 1926 [3.1]. According to this model, some of the ions in an ionic crystal move from their normal lattice points to interstitial positions due to thermal fluctuation, forming interstitial ions (or interstitials). Interstitials vibrate at their points and move to other interstitial sites by thermal fluctuation, chemical diffusion, or an applied electric field. The vacant lattice points or vacancies left by the interstitials can be occupied by other lattice point ions. As a result, vacancies also move in the crystal. These interstitials and vacancies are called the Frenkel defects. The number of interstitials in a unit volume (which is equal to that of vacancies), NF, is given as N e = NiNexp(- Ee 2KT )
(Eq. 3.1)
where N and N/are the total number of ions and interstitial positions in a unit volume, respectively, K the Boltzmann constant, T the temperature, and EF the formation energy of the Frenkel defect. The Schottky-type defect was introduced by Schottky in 1935 to explain simultaneous cationic and anionic conduction in ionic crystals [3.2]. According to this model, the same number of cationic and anionic vacancies exists in ionic crystals, and the appearance and disappearance of vacancies are considered to occur mainly at the crystal surface or dislocation face. The number of the Schottky ionic pair in a unit volume, Ns, is given as
Ns = Nexp(--2KT) Es
(Eq. 3.2)
where N is the total number of ionic pairs in a unit volume and Es the formation energy of the Schottky ionic pair. (In these equations, the thermal expansion of the crystal and the change of the frequency of lattice vibration are not considered. The number of defects increases somewhat if these two factors are taken into account; however, this increase in the number of defects is usually small.) The existence of the Frenkel or Schottky defect in a crystal can be estimated by comparing the ion radius, van der Waals energy, and dielectric constant (i.e., comparing EF and Es). The Frenkel defect usually appears when
Electrical Conduction in Ceramics
43
the radii of the ions of the crystal differ considerably, and the van der Waals energy and the dielectric constant are somewhat large. The Schottky defect often occurs when the differences between the radii of the cation and anion and their abilities to be polarized are small, and the van der Waals energy and the dielectric constant are both relatively small [3.2, 3.3]. The Koch-Wagner type defect was introduced by Koch and Wagner in 1937 [3.4]. This type of defect occurs when impurities or dopants are introduced into the lattice of the crystal. For example, when CaO is dissolved in ZrO2 crystal to form a solid solution, the substitution of the divalent Ca 2+ ion for the tetravalent Zr 4+ forms oxygen-ion vacancy defects in the ZrO2 lattice (in order to maintain the electroneutrality condition in the crystal). Similarly, oxygen-ion vacancies are also formed when a trivalent metal oxide, such as Y203 or Yb203, is dissolved in ZrO2. 3.2 DEFECTS IN FLUORIDE-TYPE OXIDES
Fluorite-type oxides are commonly ionic conductors and have been considered for use as electrolytes in SOFCs. The fluorite structure (CaF2) is adopted by a number of oxides of the general formula MO2, where M is a large tetravalent cation, e.g. Th 4+ and Ce 4+, as well as by a multitude of halides, sulfides, hydrides, and intermetallic compounds of composition AX2. The unit cell of the fluorite-type oxide has the so called M408 structure. This structure is schematically shown in Figure 3.1. In this fluorite structure, each metal ion
A
"///
A
9U
9 CATION OXYGEN ION
0
Figure 3.1. Crystal structure of a fluorite-type oxide
44
Chapter 3
is surrounded by eight oxygen ions, forming a body-centered cubic structure, and each oxygen ion is surrounded by four metal ions, forming a tetrahedral arrangement. To form the fluorite structure in MO2, the limiting (minimum) ionic radius ratio (the ratio of metal-ion radius to oxygen-ion radius) is 0.732. Under normal conditions of temperature and pressure, certain MO2 oxides do not have the fluorite structure because the ionic radius ratio condition is not satisfied; one example is ZrO2. At room temperature, ZrO2 has a monoclinic crystal structure. The monoclinic structure changes to a tetragonal form above 1170~ The fluorite structure only exists at temperatures above 2370~ However, the addition of certain aliovalent oxides stabilizes the fluorite structure of ZrO2 from room temperature to its melting point of 2680~ The fluorite structure of ZrO2 is stabilized by direct substitution of divalent or trivalent cations of appropriate size for the host lattice cation Zr 4§ In this case, lattice defects are created to preserve the electroneutrality condition in the solid solution. The probable models for structural defects in such case are: (i) an oxygen-ion vacancy model with all metal ions being fixed at their lattice points, (ii) a cation interstitial model with all oxygen ions being fixed at their lattice sites (Frenkel type), and (iii) a mixed model of (i) and (ii) (Schottky type). It is well established that the oxygen-ion vacancy model applies to stabilized ZrO2. For example, calculated and pycnometer density measurements confirm the presence of oxygen-ion vacancy defects in ZrO2-CaO systems [3.5-3.7]. The oxygen-ion vacancy model has been verified by X-ray [3.8, 3.9], neutron diffraction [3.103.12], and measurements of the diffusion coefficient of oxygen ions in ZrO2-CaO solid solutions [3.13]. Similar results have been obtained for other stabilized zirconias, cerias, and other fluorite-type oxygen-ion conductors. The presence of a high oxygen-vacancy concentration in stabilized ZrO2 gives rise to a high oxygen-ion mobility, resulting in high oxygen-ion conductivity. Oxygen-ion conduction takes place in stabilized ZrO2 by movement of oxygen ions via vacancies.
3.2.1 Defect structure of doped MO~ As mentioned above, doped M O 2 oxides such as stabilized Z r O 2 exhibit oxygen-ion conduction via oxygen-ion vacancies. However, the electrical conductivity in an oxygen-ion conductor can appear not only via oxygen-ion vacancies but also via mobile electronic charge carriers; i.e., both types of conduction (ionic and electronic) can occur simultaneously. The ionic transference number of an oxygen-ion conductor (the ratio of the ionic conductivity to
Electrical Conduction in Ceramics
45
the total conductivity) can vary depending on the surrounding gaseous environment (the oxygen partial pressure). Thus, it is possible to modify the defect structure (thus, conductivity) of an oxygen-ion conductor by changing the oxygen partial pressure. The dependence of defect structure on oxygen partial pressure is considered here for a general system, MO2-AO, assuming that the intrinsic defects in pure MO2 are of the Schottky type. Kr6ger-Vink notation is used to describe the various defects (V for vacancy, bracket for concentration, e / and h" for effective charges of electron and hole, and n and p for electron and hole concentrations, respectively). The following discussion largely follows those which have appeared in the literature [ 3 . 1 4 - 3 . 1 8 ] . The incorporation of AO into MO2 is described by the following equation: //
AO
x
= A M + Vo + O O
(Eq. 3.3)
This equation describes a situation where the M site is occupied by A, generating a doubly charged negative site, and it is necessary to generate two anion sites to maintain the crystal structure, one site being occupied by an oxygen ion and the other vacant, leaving a doubly positive charge. The incorporation of oxygen from the environment into the solid MO2 is described as
ZO 2 2
+ Vo + 2e/
...
X
Oo
9
(Eq. 3 4)
and the equilibrium constant K for the reaction is given by K-
n
-2
p-1/2
o~
(Eq. 3.5)
[Vo] The intrinsic Schottky equilibrium of the oxide MO2 is given by the following reaction" nil-
ill~l~
,M
..
+ 2 Vo
(Eq. 3.6)
The equilibrium constant K s for Eq. 3.6 is K s - [V~//I[Vo]2
(Eq. 3.7)
Chapter 3
46
The equations describing the intrinsic electronic equilibrium and its equilibrium constant Ki are as follows:
nil = h ' + e /
(Eq. 3.8)
K~ = np
(Eq. 3.9)
From these equations, the electroneutrality condition is given as
n + 4[I/~ a] + 2[A~]
=p
+
2[Vo]
(Eq. 3.10)
(i) Low oxygen partial pressure region: In the low oxygen partial pressure region, as the oxygen pressure decreases, the concentration of oxygenion vacancy will increase (to maintain the equilibrium constant K). This increase causes the metal vacancy concentration to decrease (to maintain the Schottky constant Ks). In this situation, [Vo] , [I/~//]
(Eq. 3.11)
Eventually, the concentration of oxygen-ion vacancy exceeds that of Ar~, which concentration is fixed by the dopant level. Thus, n must increase to maintain the electroneutrality condition, and accordingly, p must decrease. In this case, the electroneutrality condition given in Eq. 3.10 is reduced to
n = 2[V o]
(Eq. 3.12)
From Eqs. 3.5 and 3.12, the oxygen partial pressure dependence of oxygen-ion vacancy is obtained as
[l/'O] (4f)-IDp 02 -I/6 =
(Eq. 3.13)
The same dependence on oxygen pressure can be derived for the electron concentration. From Eqs. 3.7 and 3.13, the oxygen partial pressure dependence of the metal vacancy concentration is expressed as
Ks(4K)2taP~C
(Eq. 3.14)
From Eqs. 3.9, 3.12, and 3.13, the dependence of the hole concentration on oxygen partial pressure is given by p
=
Ki(K)IDP 1/6 2
"2
(Eq. 3.15)
Electrical Conduction in Ceramics
47
(ii) Intermediate oxygen partialpressure region: Under some intermediate oxygen pressure range, it is possible to approximate the electroneutrality condition as
(Eq. 3.16)
[Vo] = [A~]
This relationship indicates that over this intermediate oxygen pressure range, the concentration of oxygen-ion vacancies is not dependent on oxygen partial pressure, but fixed by the dopant level. By the same procedures described earlier, the oxygen partial pressure dependencies of the defects can be calculated and are given as follows:
KS
[I/Mm] -
(Eq. 3.17)
A//12 ~XMl
// -1/2p-114
n = (K[AM])
02
// p
=
(Eq. 3.18)
(Eq. 3.19)
These equations indicate that as the oxygen partial pressure increases, the concentration of the electrons decreases and that of the holes increases. On the other hand, the metal-ion vacancy concentration is independent of oxygen partial pressure and determined solely by K s and the oxygen-ion vacancy concentration. (iii) High oxygen partial pressure region: At some sufficiently high oxygen pressures, the electroneutrality condition can be approximated as
p = 2[A~]
(Eq. 3.20)
In this oxygen partial pressure range, the oxygen pressure dependencies of the anion and cation vacancies are given as
[Vo] - ~4[AM]2po~I2 KK l.2
(Eq. 3.2 I)
viaJ = ~ P o 2 rail14 16t- -Mj
(Eq. 3.22)
Chapter3
48
and the electron concentration is given by
/q
n -
(Eq. 3.23)
2[A~I As can be seen from Eq. 3.23, the electron concentration is constant in this oxygen pressure region. (iv) Very high oxygen partial pressure region: At some very high oxygen pressures (although this condition will not occur in operating ceramic fuel cells), the concentration of metal-ion vacancy becomes very large, i.e., [I,'a~//] > [A~]
(Eq. 3.24)
The electroneutrality condition can be expressed approximately as p = 4[I,;M///]
(Eq. 3.25)
For this very high oxygen pressure region, various defect concentrations are described as follows"
(4Ks) 2 [Vo] = [
KK~]
Ks
(
1/Sp-l/lO o~
16
)215Po~
(Ale" "~115(]['F2"~2/5 D 1/5 P
=
v~--sJ
~. . . .
i J
-o
2
Ki
/:-2/5 t ,~1/5p-115 /1 = .,~ ~,-"7-~__-J 9 O 4K s 2
(Eq. 3.26)
(Eq.
3.27)
(Eq. 3.28)
(Eq. 3.29)
The various defect concentrations in a MO2-AO system for various oxygen partial pressure regions are shown schematically in Figure 3.2 [3.16]. The defect structure of a fluorite oxide MO: doped with B 2 0 3 c a n be considered by the same procedures described above. The overall electroneutrality condition in this case can be expressed as shown below by assuming low defect concentrations so that Henry's law is obeyed n + 2[O~/] + [B~] = p + 2[Vo]
(Eq. 3.30)
49
Electrical Conduction in Ceramics
I
p-TYPE EMICONDUCTION iS IVERY HIGl~l HIGH
I
/
i
'.
i
Zill /
I
I
I
I
I
Z
n-TYPE IONIC CONDUCTION SEMICONDUCTION ' . . . . . . . . . . . INTERMEDIATE I LOW
f
o_t--e wI . - p o, ~i. ~ I..- I o,
,,
, (9 0-J
I I
----v-po, I
to,
-
[~"]
I
I I
I I I
I I
//
I
..I..___LOG OXYGEN
PARTIAL
PRESSURE
Figure 3.2. Variation of defect concentration as a function of oxygen partial pressure for a MO2-AO system [3.16]
Figure 3.3 shows a schematic illustration of the variation of defect concentration as a function of oxygen pressure for a fluorite-type oxide doped with trivalent metal oxide [3.17]. When the MO2 originally has the fluorite-type structure (e.g., CeO2), it has been generally accepted that the predominant intrinsic defects in the oxide are anion Frenkel defects , i 9e 9 Vo and 0//i 9
.I " = 2[v~i, 9.
l
p = tB.i p =" 2[0, ] I I -'@
[B.] = 2[v~l
I
/
..
/
I
,9
"<~o'"~
!~_
I
~-.._ .
.
.
i
,
.
.
I
[~] .
.
.
.
.
.
.
.
.
I
u
s ,,~
IJ ~
l.U 0 1.1
0
-J
<~r
P'~/ .
" 1
I .
.
.
I
;-....
o~.~,~.~
"
.
LOG O X Y G E N
PARTIAL
PRESSURE
Figure 3.3. Variation of defect concentration as a function of oxygen partial pressure for a MO2-B203 system [3.17]
50
Chapter 3
3.2.2
Conductivities of oxygen ions, electrons, and electron holes
The formation of oxygen-ion vacancies in doped MO2 oxides gives rise to oxygen-ion conduction in these solid solutions. The conduction occurs by diffusion of oxygen ions via vacancies. In general, the conduction process in an oxide ionic conductor is mixed ionic and electronic. The total electrical conductivity, a, of a fluorite-type oxide is given as o~
o = o~ + o n + or, = 2e[Vo]lXr6
+ enid,
+ eplxp
(Eq. 3.31)
where /z refers to the mobilities of the subscript species in which i, n, and p indicate ions, electrons, and electron holes, respectively. The ionic conductivity due to the migration of cations of the dopants and the host is neglected because the mobilities of the cations have been shown by diffusivity measurements to be several orders of magnitude lower than the mobility of oxygen-ion vacancy. The following discussion is given for a MO2-B203 solid solution; similar treatment can be used for MO2-AO systems. At low oxygen partial pressures, the hole concentration is relatively small, the total electrical conductivity becomes 0 = 2e[VoltXvo
(Eq. 3.32)
+ en,,
However, since the mobility of electrons is generally 104 to 108 times higher than that of oxygen-ion vacancies even at elevated temperatures, the fluorite oxide is approximated to be a pure n-type semiconductor. Therefore, the conductivity for a doped MO2 under this condition is given by the following equation: o = o n = entx n
=
p-116
e(2K)-l/31xn 02
(Eq. 3.33)
At intermediate oxygen partial pressures, the total electrical conductivity can be approximated as _ p-114 o = 2e[Vol . vo + e(2K~l)1/21.t,, 02 +
eKi(2K[B~])lr21.tpp1/42
(Eq. 3.34)
where the electroneutrality condition is
2tVol- 03 ,1
(Eq. 3.35)
51
Electrical Conduction in Ceramics
At high oxygen partial pressures, the fluorite oxide is approximated to be a pure p-type semiconductor, and the conductivity is given as o = e[~]i.tp
(Eq. 3.36)
Since the mobility of oxygen-ion vacancy is generally much lower than that of electrons or electron holes, MO2 doped with a trivalent metal oxide can only exhibit an appreciable ionic conductivity over a wide range of oxygen partial pressures when the concentration of oxygen-ion vacancy is considerably larger than n and p. Figure 3.4 shows a schematic diagram of the variation of electrical conductivity as a function of oxygen pressure for a fluorite-type oxide doped with trivalent metal oxide. For this system, the ionic conductivity is at the maximum when o, = %. The electronic equilibrium constant Ki (Eq. 3.9) can be expressed as Ki
E - np - NcNvexp(- -~T )
(Eq. 3.37)
where Eg is the band gap energy between the valence band and conduction band, and Nc and Nv the effective density of the electronic state in the conduction band and in the valence band, respectively. From Eq. 3.37, the minimum electronic conductivity, O'e(min.), is given as
E
e o~(,,,~..) = 2e(p,,pp N cNv)1r2exp(--2KT)
.,..... n-TYPE -'l L SEMICONDUCTION I
I I
I I
I I
~, I ~,(~ __
',
,
~,,"1. MIXED COND.
I I
I I I
.... ~ ~ ,-~ _ ~
I o,
I ,
_, I
,
MIXED' ~ i
i
I
I I
I I
I
I
I
I
I
I
I
I
'
I
I
I
I
'
I
I , ~
I .-I IONIC "1.. I ~'---| D O M A I N I " - ' ~ I
-.
o: p
I
I
t
p---p-TYPE I SEMICONDUCTION
I I I
I
I
I
I~LECTROLYTiC
I
P.
/
I
~
I
LOG OXYGEN
DOMAIN.
J
P, I
PARTIAL
(Eq. 3.38)
I
_,~"-,,,~io .,oi"o.,.
J I I
I
,
I
PRESSURE
Figure 3.4. Variation of electrical conductivity as a function of oxygen partial pressure for a MO2-B203 system [3.17]
52
Chapter 3
3.2.3 Defect domains The ionic domain boundaries Pp and P~ of a fluorite-type oxide are the oxygen partial pressures at which Po2 = Pp when O"i : tip, and Po2 = P~ when oi On. Within this oxygen pressure range and away from the boundaries, the oxide is considered to be an ionic conductor. (The electrolytic domain boundaries are the oxygen partial pressures where o-i "-- 1 0 0 0rp and a i = 100 cry. Within this oxygen partial pressure range, the conductivity of the oxide is exclusively ionic.) The ionic domain boundaries of a fluorite oxide can be estimated by the following procedure. The mobilities of each conducting species (ions, electrons, and holes) can be expressed by the following equations: "
-
A exp(-
An.
r
B
~" -
)
E
~" ) T~ exp(- KT
E.._
~e) T exp( - ~:T
It, -
(Eq. 3 39)
(Eq. 3.40) (Eq. 3.41)
where A~, B,, and C~, are constants that include entropy terms, AH mthe migration enthalpy of oxygen-ion vacancies, and E~,,n and E~,,p the migration energy of electrons and electron holes, respectively. Then, the conductivities are given as
aHm
~ = ~176
KT )
o ~ En~p-114 0 n = 0 n T- exp(--~---Tj o~
o
~
Ep pl/4
op = opT- exp(---~) 02
(Eq. 3.42) (Eq. 3.43) (Eq. 3.44)
where each cr~ represents conventional constants, which are assumed to be independent of Po2 and T, and
AHlro En -
Ep =
2
+ E~m
Eg + Er,~, +
AHv-o
(Eq. 3.45)
(Eq. 3.46)
Electrical Conduction in Ceramics
53
where z ~ v .~ is the oxygen vacancy formation enthalpy. At the oxygen partial pressure Po where a, = ap, the expression for Po can be obtained by solving Eqs. 3.43 and 3.44
oO
lnP o = 21n n oo p
2(E,-Ep Ir
(Eq. 3.47)
This equation defines the boundary separating predominantly n-type from p-type conductivity. The expressions for P, and Pp are obtained by setting a, = oi and (Tp =
O"i 0
lnP n = 41n(-~) - 4
(aHVo/2)+e..,,-AH,,,
Oi
lnPp = 41n(
) - 4
rT
(ant'J2) +aH'-E*-e"'"
op
(Eq. 3.48)
(Eq. 3.49)
KT
By combining Eqs. 3.34, 3.37, 3.39 to 3.46 with Eqs. 3.48 and 3.49, the ionic domain width is given as (written for MO2-B203) /22
In Pp = 4( [BM] A ,
P,,
N, NvB C ) + 4
Ee,+E..,,+E.~,-2AH,. ~r
(Eq. 3.50)
It can be seen from Eq. 3.50 that an increase in [B~I and a large Eg, E~,, or E,,p will increase the ionic domain, and an increase in Z ~ m and T will decrease the ionic domain. This suggests that oxygen-ion conducting ceramics exhibiting low values of Z~/m can be potential electrolyte candidates for SOFCs. It should be noted that oxygen-ion conductors having relatively large '~/m are less sensitive to decrease of the ionic domain with increasing temperature. In addition to the diagram shown in Figure 3.4, there is also a Pattersontype map suitable for illustrating the ionic and electrolytic domain boundaries. Figure 3.5 is an example of the Patterson map showing the domain boundaries of stabilized ZrO2 [3.19-3.21].
Chapter 3
54
t UJ
re'
up DOMAIN
/
t~ I.M
tr ix. ...i <
r
= o"
/
___
"
IONIC DOMAIN
O 0, ' /
S
tw < ix. z
UA
>X O (9 O
\
-t, = \
t , = o.5
o.aa
_J
1 / T E M P E R A T U R E --,,
Figure 3.5. Electronic, ionic, and electrolytic domains of a
MO2-B203
system [3.17]
3.2.4 Defect associations and clusters
The discussion regarding doped MO2 systems given above considers a random distribution of noninteracting defects. However, at low temperatures and even at low dopant concentrations, oppositely charged oxygen-ion vacancies and dopant cations may associate to form randomly distributed pairs, and the concentration of free oxygen-ion vacancy is determined by the association equilibrium 9 9"
II
Vo + A~ = (VoAM)
x
(Eq. 3.51)
or /
Vo
+
=
(Eq. 3.52)
At high temperatures, the oxygen-ion vacancies are most likely to be free at certain defect concentration ranges. Figure 3.6 shows the calculated temperature for the break between associated and free vacancy behavior for CeO2 doped with CaO, as a function of dopant concentration for various association energies, EA [3.22]. However, the formation of defect pairs also depends on the magnitude of the association energy. For example, the conductivity data at high temperatures for calcium-doped ThO2 in the range of dopant concentrations similar to that of CeO2 appears to indicate the association of vacancies and does not show
55
Electrical Conduction in Ceramics
ooo{ 3400
,
,
,
, ,,,
EA-0.5
,-
,
,
,v/_//
//yy
2000
,
,-
/
..
n..<
,
0.2 eV
~-
1500
,,~
1000
Ill 5OO
0 0
I
I
I
2
4
6
MOL%
8
10
CaO
Figure 3.6. Calculated break temperature between associated and free vacancies in CaOdoped Ce02 for various association energies [3.22]
break temperatures as C e O 2 does [3.23]. This can be explained by the difference in the association energy between the two compounds: the association energies (1.16 to 1.42 eV or 111.9 to 137.0 kJ/mol) of ThO2 solid solutions with calcium dopant concentrations of 1 to 7 mol % are much higher than those (0.20 to 0.50 eV or 19.3 to 48.2 kJ/mol) of C e O 2 solid solutions. At higher defect concentrations and even at high temperatures, a random distribution of defects and defect pairs may disappear. Defects may aggregate into defect clusters that become ordered or form two- or three-dimensional defects (dislocation loops, shear planes, or voids, as well as changes in the local crystal structure). As the binding energy of defect clusters has been known to increase with the number of dopant cations, the vacancies are expected to be more deeply trapped with increasing dopant concentration. Even with a random distribution of the dopant cations, local fluctuations can result in the formation of defect clusters. In these cases, the system may be described as a relatively homogeneous matrix with defect clusters or as a vacancy-free, ordered matrix with microdomains of another ordered structure. For example, in the case of stabilized zirconias, the ordered matrix is Z r O 2 and the microdomains could be sluggish long-range ordering forms of CaZr409 in the ZrO2-CaO system [3.24], and Zr3Y4012 in the ZrOz-Y203 system [3.25-3.27]. The experimentally observed decrease of oxygen-ion conductivity with increasing vacancy concentration following doping with large amounts of dopants
Chapter 3
56
is probably due to trapping of vacancies in aggregates or clusters. Trapped vacancies found in the clusters, however, are not immobile, but must overcome an energy barrier to move (by dissociation or rearrangement of clusters). This energy barrier is higher than that present in systems having only single vacancies. 3.3 DEFECTS IN PEROVSKITE-TYPE OXIDES
Oxides of the general formula ABO3 (A is a divalent or trivalent cation and B is a tetravalent or trivalent cation) belong to the class of compounds having the perovskite structure. The ideal perovskite structure is cubic. A large number of perovskite oxides are orthorhombic, rhombohedral, or tetragonal but can be approximated as cubic. The rare-earth perovskite oxides are commonly used as cathode and interconnect materials for ceramic fuel cells. For fuel cell applications, the electrical conductivity of the oxides is often enhanced by substituting acceptor- or donor-type cations for either the A or B sites. At present, the perovskite oxides commonly used in SOFCs are LaMnO3 for the cathode and LaCrO3 for the interconnect. The electrical conductivity of LaCrO3 (or LaMnO3) is considered to be due to the 3d electrons of the Cr 3+ (or Mn 3§ ions. An increase in conductivity is expected when a lower-valence ion is substituted for either the La 3§ or Cr 3+ (or Mn 3+) sites, resulting in the formation of Cr 4+ (or M n 4+) ions. A proposed defect structure of these perovskite-type oxides is discussed here as applied to a p-type perovskite REBO3 (RE is a trivalent rare-earth ion) with acceptor dopant A 2§ [3.28]. This type of defect behavior has been found to apply to magnesium-doped LaCrO3 and strontiumdoped LaMnO3 [3.29,3.30] (see Chapters 5 and 7). For simplicity, it is assumed that the p-type disorder prevails in nonstoichiometric perovskite oxide. The intrinsic Schottky equilibrium of REBO 3 is represented by nil = I / ~ + I/aa + 3 V o
(Eq. 3.53)
and the equilibrium constant Ks is given by K s = [l/R~[l/aa][Vo] 3
(Eq. 3.54)
The p-type nonstoichiometric reaction is given as
-3o 2 2
- v'g §
§ 300
§ 6h.
(Eq. 3.55)
57
Electrical Conduction in Ceramics
and as the cation stoichiometry must remain constant, the equilibrium constant for Eq 3.55 is (Eq. 3.56) When REBO 3 is doped with AO, the substitution of A 2+ for the RE 3+ site results in the formation of ARE, which possesses one effective negative charge. This charge will be compensated for either by C r 3+ ---> Cr 4+ or by the formation of oxygen-ion vacancies. Then, the electroneutrality condition is expressed as 2[Vo] + p = 6[I/d/] + [A~j
(Eq. 3.57)
The defect behavior of REBO3 doped with AO can be divided into five oxygen partial pressure regions. (i) Region I: In this very high oxygen partial pressure region, native nonstoichiometry prevails, and the electroneutrality becomes p = 6[VCB "]
(Eq. 3.58)
From Eqs. 3.56 and 3.58, the hole concentration is given as p = (36K)l/SPo/~n
(Eq. 3.59)
Since the equilibrium constant of intrinsic electronic defects, K/, equals np, the electron concentration is n =
Ki
p-3/,6
(36K) l/s
02
(Eq. 3 60) ~
and the oxygen-ion vacancy concentration is K s /3
r, -1/s [Vo] = 2.5 K 1/12"O2
(Eq. 3 61)
(ii) Region H: In this region, as both [Vo] and [1/~/] are smaller than [ARE], the electroneutrality condition becomes /
p = [A~]
(Eq. 3.62)
58
Chapter 3
Thus, [~B//]
:
g 1]2
p3/4
02
(Eq. 3.63)
[A~ 3 From Eqs. 3.54, 3.56, and 3.62, the concentration of oxygen-ion vacancy is given as follows: [Vo]
t Ksxltar A / 12p-112
= ,---~,
(Eq. 3.64)
t-~REJ- 0 2
and the electron concentration becomes n =
K. [A~E]
(Eq. 3.65)
(iii) Region IlL" As the oxygen partial pressure decreases, oxygen is lost to form oxygen-ion vacancies, and the electroneutrality condition is represented by
p + 2[Vo] = [ A ~
(Eq. 3.66)
The equations for the various defects are as follows: [A/RE] [Vo] = 2
p
n
=
__
Ki
_
r M ]'/2K''1/6 tXXREJ ""S p-l~4
~
o~
A ]1/2Tr,'1/6 "XREJ "xS p1/4
o,
[ARE]-I/2Ks 1/6p-x/a 2-1/2K -1/6 -o~
(Eq. 3.67)
(Eq. 3.68)
(Eq. 3.69)
(iv) Region IV: In this low oxygen activity region, the electroneutrality condition and the relations for p and n are given by the following equations:
2[Vo] - [A~E]
(Eq. 3.70)
K 1/3D1/4 P
~
~1"1/3 9 02 JtXS
(Eq.
3.7 1)
Electrical Conduction in Ceramics
59
and K s /3
(Eq. 3.72)
l)-1/4
n = K K 1/3" 02
(v) Region V: Eventually, with decreasing oxygen partial pressure,
B 3+
may be reduced to B2+. In this case, the reduction is the dominant reaction (with equilibrium constant KR), and the defect concentrations are given as follows" n
=
[Vo]
=
(Eq. 3.73)
(4KR)l/3Po~/6"
2 p
Ki
=
D1/6 9
o,
(Eq. 3.74)
2(4Ke) 1/3 Figure 3.7 summarizes the defect behavior in various oxygen partial pressure regions for a REBO3 perovskite doped with AO acceptor dopant. The above defect model does not take into account association of defects. However, point defects in REBO3 perovskites may not be single, unassociated, and randomly distributed. Defect models assuming formation of defect pairs have been proposed [3.31]. V
IV
III
II
e
9
",
I 9
9
tVoJ
=
9
.
"
,
9
oO
r o~
9
,
I.o
~
9
LOG
OXYGEN
P
-~.'~
*
"
r
.
,.
9
PARTIAL
= [A~]
.
9
n
-
~
9
PRESSURE
Figure 3.7. Defect concentration as a function of oxygen partial pressure for a rare-earth perovskite oxide
60
Chapter 3
3.4 CONDUCTION PROCESSES AND TRANSFERENCE NUMBERS The total conduction process in an oxide solid conductor is generally mixed ionic and electronic. Therefore, it is necessary to characterize the partial current density and transference number of each conducting species as a function of oxygen partial pressure. This section discusses general transport processes, ionic and electronic currents, and transference numbers in oxide electrical conductors. 3.4.1 General transport equations Let the partial current density carried by conducting species X be jx, the charge of X be zxq where Zx is the valence of X, q be the absolute electronic charge, the concentration of X be nx, the mobility be #x, and the diffusion coefficient associated with X be Dx. Then, jx is expressed by Jx = - n x IZx Iq~txV~ - Dx IZx IqVnx
(Eq. 3.75)
where 9 is the electrical potential. T,he electrochemical potential for X, /Xx, is given as
~tx = ~x + Izxlq~
(Eq. 3.76)
where ~x~iS the chemical potential for X as represented approximately by the following equation: !
0
Ixx - I~x + KTlnnx
(Eq. 3.77)
(nx is used instead of the activity of X.) The Nernst-Einstein equation for Dx is given by Dx -
K/'~ x IZxlq
(Eq. 3.78)
and the gradient in the electrochemical potential is expressed as _
V~x =
K/Vn x nx
+ [zxlqV~
(Eq. 3.79)
Combining Eqs. 3.75 and 3.78 yields Jx = - n x IZx Iq~txV* - ~xKrVnx
(Eq. 3.80)
Electrical Conduction in Ceramics
61
From Eqs. 3.79 and 3.80, the partial current density of species X is given by Jx = -nxl-txVlXx
(Eq. 3.81)
The conductivity of species X is given as ox =
nx~xlZxlq
(Eq. 3.82)
Thus, from Eqs. 3.81 and 3.82, the partial current density can be expressed as oxV~tx Jx - - ~
(Eq. 3.83)
Izxlq
From this equation, the partial current density for a particular species is shown to be proportional to the gradient of the electrochemical potential for that species.
3.4.2 Electronic, ionic, and total current The total current density carried by electronic species (electron or electron hole), Je, is given by j, = j,, - jp
(Eq. 3.84)
From Eq. 3.83, j, =
q
"VI~ ,, +
t, V~ p q
(Eq. 3.85)
Eq. 3.85 can be rearranged to Je = -
(O n + O p)
q
Vp. n + Op( -.~n + -~p)
q
(Eq. 3.86)
Assuming that the thermodynamic equilibrium between electrons and holes is not disturbed by the flow of particles, the following equation is established: V~ n + Vlsp = 0
(Eq. 3.87)
Thus, j~ = _
(O +Op n q
7-~',,
(Eq. 3.88)
62
Chapter 3
Since tr~ = tr~ + trp, the electronic current density is given as m
o ~V_,, -u - o .Vi.t p q q
(Eq 3.89)
Similarly, the ionic current density is given by j, = - (~176 Iz lq
= (~176
lq
V~I
(Eq. 3.90)
where the subscripts 1 and 2 represent the cations and anions, respectively. The total current density is given as j = j, + j , =
ff
q
--
"Vl~p
0 i
Iz lq
V-~x
(Eq. 3.91)
where X is one of the various species in the specimen by which the thermodynamic equilibrium is expressed as x
+ [z lh" = x
(Eq. 3.92)
3.4.3 Transference number measurements Solid oxide electrical conductors are generally mixed electronic and ionic conducting materials. Under specified conditions, whether an oxide is ionic, electronic, or mixed conducting depends on the relative magnitude of the ionic transference number ti (including cation and anion contributions) and the electronic transference number t~ (the sum of the electron and electron hole transference numbers, t~ + tp). Evaluation of transference numbers of an oxide conductor is important in the selection of a material for use as a SOFC electrolyte, electrode, or interconnect component. For fuel cell applications, the transference number of ions must be above 0.99 and that of electrons below 0.01 for electrolyte, and a large transference number of electrons is desired for electrode materials. For example, (ZrO2)0.8: (CaO)0.15 is an ionic conductor suitable for SOFC electrolyte application. With P02 = 1 atm (105 Pa) on one side and Po2 = 2 • 10-~ to 10-17 atm (2 • 10 4 to 10 -~2 Pa) on the other side, the material has an ionic transference number of 0.998 to 0.994 at 1000 oc [3.32]. Ionic transference numbers can be determined using oxygen gas concentration cells. For example, in the concentration cell shown below
Electrical Conduction in Ceramics
63
(Eq. 3.93)
Fe, FeO J (ZrO:)o.85-(CaO)o.,, ] Cu:O,Cu
the oxygen pressures at the anode and cathode are determined by the equilibriums FeO ~ F e + %02 CuO ~ 2Cu + 1/202
(Eq. 3.94) (Eq. 3.95)
By this oxygen concentration method, the ionic transference number of (ZrO2)0.85(CaO)0.15 has been found to be 0.997 at 700 ~ and 0.996 at 800~ [3.33]. Figure 3.8 lists some fluorite-type oxygen-ion conductors which exhibit oxygen-ion transference numbers above 0.99 at 1000~ as a function of composition and oxygen partial pressure [3.34]. In an oxygen gas concentration cell, the electromotive force, dE, of the cell is given by (Eq. 3.96)
d E / = ti(-~)dlnPo~ q
02. TRANSFERENCE NUMBER > 0.99 ( 1000 oC) COMPOSITION MOL%
~. =,
0
~o
~
~
o~
o o
0 7 ~7 7, ~ '7, ZrOz-CaO (85:15)
-
ZrO2-Y016 (80:20)
,
I
,
~_
.
0
~,
z =o
,.;~oII
I
{
I
[
I
[
, I
t I
'
I =
I
I
[
I
1
I
I
I
I
,
I
I
i ThO2-Y016 (99:1 ) i
ThO2-Y01.5 (96:4) "
I I
ThO2-Y016 (90:10) ThOz-YOl.s (85:15)
I I
I I
i171l i
ThO2-La01.6 (90:1 O} ThO2"La01.6 (85:15]
I I f
Tho2-LaO, 5 (75i2r~)I
; Tho,-c"o
]
.
0 5 10 15 20 25 -LOG OXYGEN PARTIAL PRESSURE, atm (1.01 x 10 ~ Pa)
Figure 3.8. Oxygenpartial pressure range for fluorite-type conductors exhibiting oxygen-ion transference numbers > 0.99 at IO00~ [3.34]
64
Chapter 3
Then, the measurable electromotive force of the concentration cell is given as E / = KTi~~ 4q J tta'o~,~
(Eq. 3.97)
Differentiation of Eq. 3.97 with respect to lnPo2 yields the following relation for the ionic transference number: 4q aE / ti = KT 01nPo2
(Eq. 3.98)
This equation shows that the ionic transference number can be obtained experimentally at any oxygen partial pressure from the slope of the curve of the electromotive force versus lnPo2 at that oxygen pressure. Thus, in the case of fuel cells, by plotting E / (obtained at the same cathode oxygen pressure, Po2c~), and different anode oxygen pressures, PO2(a),) against lneo2(a), t i can be obtained as a function of PO2(a). By this type of measurement, t i has been found to be almost unity over wide oxygen pressure ranges for stabilized zirconia at elevated temperatures [3.5, 3 . 1 0 , 3 . 3 5 , 3.36]. In certain cases, it may be necessary to determine the value of t~ directly (instead of evaluating it by 1 - O, especially when the value of t e is small (as in the case of SOFC electrolytes). In SOFCs, even under open-circuit conditions, currents continue to flow so long as their sum is zero. In such conditions, the particles move via chemical diffusion. According to ambipolar diffusion theory [ 3 . 3 7 , 3 . 3 8 ] , the chemical or ambipolar diffusion coefficient, Da, in mixed conductors is given as D a = teD i + t i d e
(Eq. 3.99)
where D i and D e are the oxygen ion and electronic diffusion coefficients, respectively. When ti ~ te (i.e., for predominantly ionic conductors), D a = tiD e = D e
(Eq. 3.100)
The two experimental methods most commonly used to evaluate small electronic contributions in an oxide conductor are the permeation [3.35] and polarized cell [3.39] techniques. (i) P e r m e a t i o n t e c h n i q u e : When a fixed gradient of oxygen pressure is maintained across a specimen, a steady state flux of neutral oxygen flows from
Electrical Conduction in Ceramics
65
the high oxygen pressure side to the low oxygen pressure side. The oxygen flux, Jo, is given by the following equation:
Jo = -Da~Co
(Eq. 3.101)
where Co represents the concentration of oxygen. By using Eq. 3.100, expressing the Wagner scaling equation in terms of conductivities [3.36], and introducing KTInP for the chemical potential of neutral species, the permeation current density, j, is given by KT J = 4q o ~t~VInPo~
(Eq. 3 102)
Integration over the sample thickness, L, leads to KT
tin/,//
j = ~O4qL ~J~,, tedlnPo2
(Eq. 3.103)
where P / and P Hare oxygen pressures at the high-pressure side and a fixed lowpressure side of the permeation cell, respectively. For the evaluation of the transference number, t~, at a certain oxygen pressure of P, it is useful to differentiate Eq. 3.103 with respect to the upper integration limit to obtain
OlnPo~ eo, -ell --
o i t~
(Eq. 3.104)
From the relation above, te at P can be evaluated in terms of the slope of the plot of experimental permeation current densityj versus lnP". It should be noted that this analysis has no restrictions and can be used even when the dependence of ore on oxygen partial pressure (electronic conductivity being n- or p-type) is not known. (ii) Polarized cell technique: Partial electronic conductivities can also be determined by using ion-blocking electrodes to suppress ionic transport so that only electrons and electron holes can pass through the system. This is accomplished by using a chemically inert material, like Pt or Au, as a blocking electrode (the cathode in this case), so that no ions are supplied to the specimen when a DC voltage, E, (below the decomposition voltage of the sample material) is applied. An electrode that is reversible to ionic species is used as the counter electrode (the anode) to fix the chemical potential of the components. In this case, conduction takes place only by the migration of electronic carriers.
Chapter 3
66
Assuming that the electronic carriers are dilute enough to obey ideal solution la~ and to have a constant mobility [3.39], the following equation has been derived: (Eq. 3.105)
i _ exp(_~T)
~[
P
~:lJ
where a~/ and a/represent the electron and hole conductivities in chemical potential determined by the reversible electrode. Then, a plot of the left side of Eq. 3.105 versus exp(qE/KT) should give a straight line. The electron and hole conductivities are obtained from the slope of the plot and from the intercept with the ordinate, respectively [3.40]. The key technical challenge in this technique is to have satisfactory blocking conditions. However, it has been demonstrated that even though blocking of the ionic flow is incomplete, the polarized cell treatment discussed above describes well observed experimental data [3.41]. The techniques described above are static methods; in addition, the application of these techniques under dynamic conditions using transient measurements has been demonstrated. For example, if the applied voltage is removed after attaining a steady state, the concentration gradients will decay until equilibrium concentrations are reached. These transients will show measurable voltage relaxations. From the time dependence of these voltage relaxations, expressions for diffusion coefficients of electrons and electron holes can be obtained [3.42-3.44]. (iii) Other techniques: There are also many other techniques for determining transference numbers [3.35,3.40,3.45-3.47]. For instance, the electron and electron hole contributions are evaluated by subtracting the oxygen pressure independent component from the total conductivity at a certain oxygen partial pressure [3.40,3.45,3.46]. The transference number of a conducting species may be determined by measuring its self diffusion coefficient, calculating its conductivity, and comparing the calculated conductivity with the total conductivity [3.35]. The individual contributions of anions, cations,and electrons to the total conductivity may be evaluated by electrolysis experiments. The thermoelectronic emission from oxides at elevated temperatures has been found to be useful to identify electronic contributions, since the emission flux is sensitive only to the electron density [3.47].
Electrical Conduction in Ceramics
67
References 3.1 3.2 3.3 3.4 3.5 3.6 3.7 3.8 3.9 3.10 3.11 3.12 3.13 3.14 3.15 3.16 3.17
3.18
3.19 3.20 3.21 3.22 3.23 3.24 3.25 3.26 3.27
J. Frenkel, Z. Phys. Chem., 35 (1926) 652. W. Schottky, Z. Phys. Chem., 29B (1935) 335. W. Jost, J. Chem. Phys., 1 (1933)466. E. Koch and C. Wagner, Z. Phys. Chem., 38B (1937) 295. F. Fund, Z. Elektrochem., 55 (1951) 363. F. Fund, Z. Phys. Chem., 199 (1952) 142. C. Wagner, Naturwissenschaften, 31 (1943) 265. T.Y. Tien and E.C. Subbarao, J. Chem. Phys., 39 (1962) 572. H. Schmalzried, Z. Elektrochem., 66 (1962) 572. R.E. Carter and W.L. Roth, G.E. Research Report No. 63-RL-3479M, General Electric, Schenectady, NY, 1963. J. Faber, Jr., M.A. Seitz, and M.H. MOiler, J. Phys. Chem. Solids, 37 (1976) 903. J. Faber, Jr., M.A. Seitz, and M.H. MOiler, J. Phys. Chem. Solids, 37 (1976) 909. W.D. Kingery, J. Pappis, M.E. Doty, and D.C. Hill, J. Am. Ceram. Soc., 42 (1959) 393. C.B. Choudhary, H.S. Maiti, and E.C. Subbarao, in Solid Electrolytes and Their Applications, E. C. Subbarao (ed.), Plenum Press, New York, 1980, p. 1. E.C. Subbarao and H.S. Maiti, Solid State lonics, 11 (1984) 317. C.A.C. Sequeira and J.M.B.F. Diniz, Phys. Status Solidi A, 165 (1988) 123. O.T. Sorensen, 0. Johannesen, and K. Clausen, in Transport-Structure Relations in Fast Ion and Mixed Conductors, F.W. Poulsen, N.H. Andersen, K. Clausen, S. Skaarup, and O.T. S~rensen (eds.), Ris~ National Laboratory, Roskilde, Denmark, 1985, p. 93. 0. Johannsen, in Proceedings of International Energy Agency Workshop on Mathematical Modelling of Natural Gas Fueled Solid Oxide Fuel Cells & Systems, July 2-6, 1989, Charmey, Switzerland, Swiss Federal Office of Energy, Bern, Switzerland, 1989, p. 99. L. Heyne and D. Engleson, J. Electrochem. Soc., 19 (1977) 727. H.L. Tuller, in Nonstoichiometric Oxides, O.T. Sorensen (ed.), Academic Press, New York, 1981, p. 271. J.W. Patterson, in Electrical Conductivity in Ceramic and Glass, Part B, N.M. Tallan (ed.), Marcel Dekker, New York, 1974, p. 453. A.S. Nowick and D.S. Park, in Superionic Conductors, G.D. Mahan and W.L. Roth (eds.), Plenum Press, New York, 1976, p. 395. H.S. Maiti and E.C. Subbarao, J. Electrochem. Soc., 123 (1976) 1713. B. Hodson and P.T. Moseley, J. Solid State Chem., 19 (1976) 383. S.F. Bartram, Inorg. Chem., 5 (1966) 749. M.R. Thornber, D.J.M. Bevan, and J. Graham, Acta Cryst. B, 24 (1968) 1183. S.P. Ray and D.E. Cox, J. Solid State Chem., 15 (1975) 333.
68
3.28
3.29
3.30 3.31 3.32 3.33
3.34 3.35 3.36 3.37 3.38 3.39 3.40 3.41 3.42 3.43 3.44 3.45 3.46 3.47
Chapter 3
H.U. Anderson, in Proceedings of the 14th Riso International Symposium on Materials Science, High Temperature Electrochemical Behaviour of Fast Ion and Mixed Conductors, September 6-10, 1993, Roskilde, Denmark, F.W. Poulsen, J.J. Bentzen, T. Jacobsen, E. Skou, and M.J.L. OstergArd (eds.), Riso National Laboratory, Roskilde, Denmark, 1993, p. 1. H.U. Anderson, J.H. Kuo, and D.M. Sparlin, in Proceedings of the First International Symposium on Solid Oxide Fuel Cells, October 16-18, 1989, Hollywood, FL, S.C. Singhal (ed.), Electrochemical Society, Pennington, NJ, 1989, p. 111. H.U. Anderson, Solid State Ionics, 52 (1992) 33. P. Kofstad and A. Petrov, see Ref. 3.28, p. 287. J. Weissbart and R. Ruka, in Fuel Cells, Vol. II, G.J. Young (ed.), Reinhold, New York, 1963, p. 37. S.F. Pal'guev and A.D. Neuimin, in Transactions (Trudy) of the Institute of Electrochemistry No. 1, Electrochemistry of Molten and Solid Electrolytes, Consultants Bureau, New York, 1961, p. 90. B.C.H. Steele and C.B. Alcock, Trans. Metall. Soc. AIME, 233 (1965) 1359. L.A. Simpson and R.C. Carter, J. Am. Ceram. Soc., 49 (1966) 139. K. Kiukkola and C. Wagner, J. Electrochem. Soc., 104 (1961) 379. W. van Roosbroeck, Phys. Rev., 91 (1953) 282. L. Heyne, in Solid Electrolytes, S. Geller (ed.), Springer-Verlag, New York, 1977, p. 169. C. Wagner, in Proceedings of the 7th Meeting of C.LT.C.E., 1955, Lindau, Germany, Butterworths Scientific, London, U.K., 1957, p. 361. J.W. Patterson, E.C. Bogren, and R.A. Rapp, J. Electrochem. Soc., 114 (1967) 752. D.Y. Wang and A.S. Nowick, J. Electrochem. Soc., 127 (1980) 752. W. Weppner, Z. Naturforsch. A, 31 (1976) 1336. L. Heyne and N.M. Beekmans, Proc. Br. Ceram. Soc., 19 (1971) 229. K. Kitazawa and R.L. Coble, J. Am. Ceram. Soc., 57 (1974) 360. H.L. Tuller and A.S. Nowick, J. Electrochem. Soc., 122 (1975) 255. T. Takahashi, H. Iwahara, and T. Esaka, J. Electrochem. Soc., 124 (1977) 1563. J.C. Rifflet, P. Odier, A.M. Anthony, and J.P. Loup, J. Am. Ceram. Soc., 58 (1975) 493.
Chapter 4 ELECTROLYTE 4.1 REQUIREMENTS The main function of the SOFC electrolyte is to conduct ions between the anode and cathode. The electrolyte carries the ions produced at one electrode to the other electrode to balance the charge from the electron flow and complete the electrical circuit in the fuel cell. The conducting ion must be or contain one of the elements present in the fuel and/or oxidant. The electrolyte also separates the fuel from the oxidant in the fuel cell. Thus, the electrolyte material must be stable in both the reducing and oxidizing environments, impermeable to the reacting gases, and sufficiently conductive (ionically) at the operating conditions. Since the SOFC operates at high temperatures (600 ~ to 1000~ the electrolyte must be chemically and thermally compatible with the other cell components from room temperature to those operating temperatures, and to even higher temperatures at which the fuel cell is fabricated. The key requirements for the electrolyte in the SOFC are discussed below. This discussion is qualitative because the specific requirements depend on selected materials and cell and stack designs [4.1]. (i) Stability: The electrolyte must be chemically, morphologically, and dimensionally stable in the dual atmosphere (reducing atmosphere on one side and oxidizing atmosphere on the other). It may not experience any disruptive phase transformation (involving large changes in molar volume) between room temperature and fabrication temperature. (ii) Conductivity: The electrolyte must possess adequate ionic conductivity in the dual atmosphere (at the fuel cell operating temperature); its ionic conductivity must be as high as possible to minimize ohmic losses. The electrolyte must also have negligible electronic conductivity to prevent voltage losses due to the electronic current flowing through the electrolyte. The electrolyte conductivity must not change (age) significantly over prolonged periods.
Chapter 4
70
(iii) Compatibility: The electrolyte must be chemically compatible with the other cell components, not only at the operating temperature, but also at the much higher temperature at which the fuel cell ceramic structure is fabricated. The electrolyte is typically the first component considered in the construction of the SOFC. Therefore, other cell materials must be selected to limit chemical interaction and elemental diffusion between the electrolyte and the other components in order to minimize unacceptable occurrences such as insulating phase formation, stability reduction, change in thermal expansion, introduction of significant electronic conductivity in the electrolyte, etc. (iv) Thermal expansion: The thermal expansion of the electrolyte must match (from room temperature to operation and fabrication temperatures) that of other cell components to avoid cracking and delamination during fabrication and operation, including thermal cycling. The coefficient of thermal expansion of the electrolyte material must remain unchanged despite changes in oxygen partial pressures of the fuel and oxidant atmospheres during operation. The electrolyte is typically selected as the baseline material, and the thermal expansion characteristics of other materials are tailored to match those of the electrolyte. (v) Porosity: The electrolyte must be dense (or contain no connected porosity) to prevent gas cross leakage. The electrolyte material must be impervious to both oxidant (oxygen) and fuel (hydrogen) gases between room temperature and operating temperature. In addition to these requirements, other desirable properties for the SOFC electrolyte are high strength and toughness, fabricability, and low cost. Present SOFCs use, almost exclusively, stabilized zirconia (ZrO2), especially yttria (Y203)-stabilized ZrO2 (YSZ), as the electrolyte. Other oxygenion conductors (such as doped CeO2, stabilized Bi203, and other conducting oxides) have also been proposed as electrolyte materials for the SOFC, especially for reduced-temperature operation (600 ~ to 800~ In addition, a number of proton-conducting oxides have been studied for use as SOFC electrolytes. 4.2 STABILIZED ZIRCONIA Stabilized ZrO 2 has been used almost exclusively as the electrolyte in SOFCs because the material possesses an adequate level of oxygen-ion conductivity and exhibits desirable stability in both oxidizing and reducing atmospheres. Among the various stabilized zirconias, the Y203-stabilized material is the most common.
Electrolyte
71
4.2.1 Preparation In SOFCs, the stabilized ZrO2 electrolyte is generally fabricated as a polycrystalline dense film or layer. Various processes have been developed to make thin ZrO2 electrolyte layers for the SOFC (see fabrication sections of Chapter 9 for more details). These processes are based on either the particulate approach or the deposition (including coating) approach. The particulate approach involves compaction of ZrO2 powder into the desired shape, and densification at elevated temperatures. Examples of the particulate approach are tape casting and tape calendering. The deposition approach involves the formation of a thin layer (on a substrate or support) by a chemical or physical process. Examples of the deposition approach are electrochemical vapor deposition (EVD) and plasma spraying. The most important aspect in the fabrication of the electrolyte is the production of a fully dense layer (as thin as possible). In the particulate approach, the densification of powder at elevated temperatures is dependent on material and processing factors, such as powder characteristics (reactivity, purity, morphology), particle packing (green density), and processing conditions (temperature, time, atmosphere). Ideally, fine (high surface area) spherical particles with a narrow size distribution are desirable because they result in high reactivity and high packing density, and therefore, enhanced densification of powders (into sintered bodies with uniform microstructure) at low sintering temperature. At present, ZrO2 powders with such characteristics can be prepared and have been processed into dense layers under conditions suitable for SOFC fabrication. Recently, further advancements have been made in powder synthesis and processing of ZrO2 materials. For example, YSZ powders of submicrometer size (nanocrystalline size) have been formed into a green body (about 50 % green density) and fired to 95 % theoretical density in air at 1125~ [4.2]. Microwave sintering has been demonstrated to densify ZrO2 powders at reduced temperatures [4.3] and shorter hold times [4.4]. For SOFC applications, common particulate methods are tape casting [4.5,4.6] and tape calendering [4.7,4.8]. Tape calendering is also suitable for making pinhole-free, micrometer-thick YSZ electrolyte layers for reduced-temperature operation [4.9]. Figure 4.1 shows an example of the microstructure of YSZ electrolyte made by tape calendering, a particulate method.
72
Chapter 4
Figure 4.1. Microstructure of YSZ electrolyte made by tape calendering
In the deposition approach, the electrolyte is commonly formed as a thin layer on a substrate or support. The key consideration in this approach is the ability of the method to produce a dense and pinhole-free layer. Therefore, process parameters of selected methods are often tailored to achieve this requirement. At present, the common deposition methods for the SOFC are EVD [4.10] and plasma spraying [4.11]. Many other deposition methods have also been proposed and investigated, including chemical vapor deposition (CVD) [4.12], rf sputtering [4.13], rf ion plating [4.14], spray pyrolysis [4.15], slurry coating [4.14], vapor-phase electrolytic deposition [4.16], CO2 laser evaporation [4.17], laser spraying [4.18], pulse laser deposition [4.19], sol-gel coating [4.20], plasma enhanced metal organic CVD [4.21], jet vapor deposition [4.22], electrophoretic deposition [4.23], vacuum evaporation [4.24], and hybrid plasma spraying [4.25]. Several of these techniques have been studied for making electrolyte layers thinner than 10/zm (see Chapter 9, section 9.5.3 for further details and more references). In the particulate methods discussed above and certain deposition techniques, ZrO2 precursor powders containing a desired amount of stabilizing oxide are required. The ideal powder should be homogeneous (having the stabilizing additive uniformly distributed on an atomic scale), yet large enough to handle, while the surface area should be sufficiently high to allow sintering at the lowest possible temperature [4.26]. A wide range of stabilized ZrO2 powders have been produced by various methods (Table 4.1) [4.27]. At present, highly reactive and uniform ZrO2 powders are commercially available. Figure 4.2 shows the steps of a manufacturing process based on hydrolysis of ZrOC12 and
Electrolyte
73
TABLE 4.1 Characteristics of Powders Produced by Various Preparation Methods [4.27]
Method
Calcining temperature (~
Agglomerate size (~m)
Tap density (% theor.)
Surface area (mZ/g)
Hot kerosene Citrate Sol-gel microsphere Peroxide Acetone-toluene Alkoxide Chloride
600 650 650 600 650 650 650
2-20
18 5 26 38 32 12 10
4 58 32 82 16 90 123
1-20 <__50 ___100
ZIRCON SAND (ZrO2SiO2)
Y203
Na2ZrO3Na2SiO3 ZrOCI2-HCI
ZrOCI2"8H20 SOLUTION
CHLORIDE SOLUTION HYDROLYSIS CALCINATION
MILLING SPRAYING YSZ POWDER
Figure 4.2. A manufacturing process for producing YSZ powder
74
Chapter 4
YC13 to produce fine YSZ powders. As ZrO2 powders are generally prepared from chloride precursors, these materials may contain chloride residue. The presence of a significant amount of chloride (1 wt%) can raise the sintering temperature of the material as much as 150~ [4.28,4.29]. If necessary, laundering techniques can be used to remove the chloride impurity [4.28, 4.29].
4.2.2 General properties and phase transformation
ZrO2, in its pure form, exhibits three well-defined polymorphs. At room temperature, ZrO2 has a monoclinic crystal structure. The monoclinic structure changes to a tetragonal form above 1170~ and to a cubic fluorite structure above 2370~ The monoclinic/tetragonal transformation in ZrO2 is thermodynamically reversible but associated with a large volume change (3 to 5%) (contraction on heating and expansion on cooling). The cubic phase exists up to the melting point of 2680~ However, the addition of certain aliovalent oxides can stabilize the cubic fluorite structure of ZrO2 from room temperature to its melting point. Table 4.2 lists several properties of ZrO2. The properties of stabilized ZrO2 have been extensively studied [4.30-4.33], and several reviews on the subject are available [4.34-4.36]. The common stabilizing oxides for ZrO2 are CaO, Y203, MgO, Sc203, and certain rare-earth oxides. These oxides exhibit a relatively high solubility in ZrO2 and are able to form various solid solutions with ZrO2, including cubic fluorite solid solutions which are stable over wide ranges of composition and temperature. Figure 4.3 shows the equilibrium phase diagram for the ZrO2-CaO system (where M~, Ts~, and C~s indicate monoclinic, tetragonal, and cubic solid solution, respectively) [4.37]. The system has a eutectoid at about 17 mol % CaO in the composition range CaO-CaZrO3. From 6 to 17 mol% CaO, the material (known as partially stabilized ZrO2) consists of tetragonal solid solution and monoclinic solid solution phases above 1140 ~ Slow cooling from 1140 ~ to 1000~ results in the tetragonal solid solution phase and CaZr409 (the eutectoid decomposition product). Further cooling below 1000~ causes the martensitic transformation of the tetragonal solid solution to monoclinic solid solution. The cubic phase is thermodynamically unstable at low temperatures. The eutectoid decomposition of cubic solid solution occurs at 1140~
Electrolyte
75
T A B L E 4.2
Properties of ZrO2
Melting point, ~ Density, g/cm 3 Undoped ZrO 2 (monoclinic) YSZ (8 mol% Y203) Electrical conductivity, f~-lcm-~ YSZ (9 mol% Y203) (1000~ YSZ (9 mol% Y203) (600~ Thermal conductivity, W/cm.K Thermal expansion coefficient, cm/cm.K Undoped ZrO2 (20 ~ to 1180~ YSZ (8 mol% Y203) (100 ~ to 1000~ Standard enthalpy of formation (25~ kJ/mol Standard entropy of formation (25~ J/mol.K Bend strength, MPa YSZ (8 mol% Y203) at 25~ YSZ (8 mol% Y203) at 1000~ Fracture toughness at 25~ (YSZ), MN'm -3/2
2680
[4.34]
5.56 5.90
[4.34] [4.34]
0.12 0.006 0.02
[4.36] [4.36]
8.12 10.8 -1,097.5 50.4
[4.106] [4.110]
300 225 3
[***]
[*]
[**] [**]
[4.118] [***]
[*] from brochure of Vesuvius Mc Danel, Beaver Falls, PA [**] from JANAF ThermochemicalTables, Third Edition, American Institute of Physics, New York [***] from brochure of Tosoh Corporation, Tokyo, Japan
"" ...
2 2 5 0 + 2 0 "C
~ - -
"
0 o
zooo
u~ n,=) I--
T
lss
ss
r
uJ n
Css
Css
t-
CaZr03
Css 1500
gJ I--
Tss '*
0000' 9
Mss
.
oo
,
9 9
9 9
1310 -4- 4 0 " C Css +
iooo
9
_,,. .
[,
t"
0
ZrO 2
.
.
.
.
.
.
Mss
CaZr 4 09
.
.
c.z,o 9 o~
.
"P C e Z t 4 0 9
i I0
"/ 30
20
MoI%
m 40
50
C0ZrO$
CeZr 4 0 9 CaO
Figure 4.3. Phase diagram of a ZrOz-CaO system [4.37]
Chapter 4
76
For the ZrO2-Y203 system, several equilibrium phase diagrams have been reported (and certain discrepancies still exist). Figure 4.4 shows a phase diagram of the ZrO2-Y203 system [4.38]. The diagram of the low Y203 region is given in Figure 4.5 [4.39, 4.40]. It can be seen from Figure 4.5 that the addition of Y203 to ZrO 2 reduces the temperature of the tetragonal/monoclinic transformation, and the transformation temperature decreases with increasing Y203 content (in the composition range 0 to 2.5 mol % Y203). In this composition range, the tetragonal solid solution is transformable, i.e., the tetragonal phase will transform on cooling to the monoclinic phase. At higher Y203 contents, a mixture of nontransformable tetragonal and cubic solid solutions exists. Further increase in Y203 content results in a homogeneous cubic solid solution. The minimum Y203 amount required to fully stabilize the cubic phase of ZrO2 is about 8 to 10 mol % at 1000~ [4.38,4.39,4.41]. The ZrO2-MgO has a eutectoid at 13 mol% MgO [4.37]. A cubic solid solution exists at this composition above 1400~ The cubic solid solution decomposes into a tetragonal solid solution and MgO below 1400~ and again into a monoclinic solid solution and MgO below 1240~ Other ZrO2-M203 systems (where M is ytterbium, scandium, neodymium, samarium, or gadolinium) have also shown stabilized solid solutions in a certain M203 range [4.42-4.51]. The minimum amount of M203 necessary to stabilize ZrO2 in cubic structures is close to the composition which gives the highest conductivity (approximately 8 mol % for Yb203, 10 mol % for Sc203, 15 mol % for Nd203, 10 mol % for Sm203, and 10 mol % for Gd203).
4.2.3 Stability ZrO 2 is chemically stable in the SOFC oxidizing and reducing atmospheres. Only under highly reducing conditions, e.g., below 10.25 to 10.30 atm (10 .20 to 10.25 Pa) at 1000~ (not normal SOFC conditions), ZrO2 is blackened (reduced) by forming a zirconia suboxide, ZrO2_~. The black coloration has been ascribed to entrapped electrons [4.52, 4.53]. The reduction or blackening of ZrO2 can also be produced if a current density higher than the limiting current densities (associated with the gas electrode reactions) is forced through the electrolyte. Pure ZrO2 does not serve as a good electrolyte because its ionic conductivity is too low, and it has disruptive phase transformations on heating and cooling. Doping ZrO2 with a certain divalent or trivalent oxide can stabilize the cubic fluorite phase and, at the same time, increase its oxygen vacancy concentration. This enhances the ionic conductivity and extends the oxygen partial
Electrolyte
3000 r
~
~
77
1
-
!
i
I
r i
] i
"~ ~ ~ . . ~
'~-~ ~
F
20001 oo ui
...
t
Fr~
U
F=+C=
er"
| {
13!!oc
I--
<
11= W
~s= ~
i
o
,
1377:1: 5=C \ \ \ \
I--
\ \ \
'" i 1000
I I |
!
\
I I / Fs= / +
o
\ \
\
Z%Y4Otz
+
\
Cs=
r,,,, +o~\o /z,.~.o,. s= | ~r \\
\
ii
'iI
\ / Ms= + Z%Y,Otz h ~ 2"0
Zr02
,
, 40
~ 80
60
, Y203
Mol % Y203
Figure 4.4. Phase diagram of a ZEO2-Y203 system [4.38]
ooot
I
T
I
LIQUID
2500
{-) 2000 o
er
1500 I.U I.U I--
1000
500
0 ~ - .
0 z~o~
(6%)
5
TET ( 1 1 % _ ) _ _ ~ 10
Mol % YO 1.s
15
,. 20
~12(Y2O3)---
Figure 4.5. Phase diagram of a ZFO2-Y203 system in the low }'203 region [4.39]
Chapter 4
78
pressure range of ionic conduction, making stabilized ZrO2 suitable for use as an electrolyte in SOFCs. (This extended oxygen partial pressure range covers the conditions, 1 to 10-17 atm (105 to 10-~2 Pa), to which a SOFC electrolyte is exposed in the operating fuel cell.) In general, fully stabilized ZrO2 is preferred as SOFC electrolyte material in order to maximize conductivity. The use of fully stabilized ZrO2 also avoids the problems of phase transformation and conductivity aging associated with partially stabilized materials during cell operation.
4.2.4 Electrical conductivity ZrO2 stabilized with a cation of appropriate size is an oxygen-ion conductor. ZrO2 is stabilized by direct substitution of divalent or trivalent cations for the host lattice cation Zr4§ This substitution creates a large concentration of oxygen vacancies by charge compensation according to following equation (written for Y203 stabilization using Kr6ger-Vink notation): ZrO2
y~o3
_. 2y/z, + Vo + 300
(Eq. 4.1)
The high oxygen vacancy concentration gives rise to high oxygen-ion mobility. Oxygen-ion conduction takes place in stabilized ZrO2 by movement of oxygen ions via vacancies. The general features of the defect structure and oxygen-ion conduction in stabilized ZrO2 are discussed in detail in Chapter 3. The ionic conductivity of stabilized ZrO2 has been extensively studied and measured. The ionic conductivity behavior of the material is influenced by several factors such as dopant and dopant concentration, temperature, atmosphere, grain boundary, and time. (i) Conductivity measurement: Complex impedance measurements are commonly used to determine the ionic conductivity of stabilized ZrO2. It is well established that ionic conductivity of polycrystalline ZrO2 (and ceramics in general) depends on the microstructures, especially grain boundaries, of the material. The complex impedance method has also been used to separate the contributions of grain boundaries to the total conductivity (resistivity) [4.545.57]. Analysis of impedance data often employs equivalent circuits to elucidate the contributions of grain boundaries. The individual components of the equivalent circuit are related to parameters of the resistivity such as the bulk or grain interior resistance (Rgi) and capacitance (Cgi) and the grain-boundary resistance (Rgb) and capacitance (Cgb). Figure 4.6 shows, as an example, two equivalent circuits for polycrystalline ZrO2 [4.58]: one showing impedance
Electrolyte
Rgi
]
~gb
R~
Cgi
c~o
c~
Rb
r
t
fe
. IN
Cb
79
fg
FREQUENCY
Rgi - - - 4 " - - -
Rgl, ~ - 4 - ' ~
Re F---
R~
Re Z/, ~
c~
"-I ---"-
Ce
Figure 4.6. Equivalent circuits and schematic complex impedance plot of polycrystalline Zr02 [4.581 components arising from grain interiors (gO, grain boundaries (gb), and electrodes (e) [4.59] and one showing parallel connection of geometric capacitance (Cg) and nonblocked (R~) and blocked (Rb, Cb) ionic paths [4.60]. A complex impedance plot of the imaginary (Z//) vs. the real (Z t) components for these equivalent circuits (over a wide range of frequencies) results in three semicircles (Figure 4.6). The diameter of each semicircle is the resistance of the corresponding circuit element. The high-frequency semicircle provides the bulk resistance and capacitance of the interior of the grains; the intermediate-frequency semicircle provides the grain-boundary resistance and capacitance; and the low-frequency semicircle provides information on the oxygen-ion transfer at the electrodes. (In practice, circular arcs rather than semicircles are often observed because the structure of actual grain boundaries is obviously more complex than that envisaged in the equivalent circuit.) It should be noted that the influence of grain boundaries on conductivity may vary depending on temperature. As a result, the complex impedance plot (number and size of semicircles) may also vary with temperature. Figure 4.7 shows an example of a complex impedance plot for ( Z r O 2 ) o . 9 ( Y 2 0 3 ) o . 1 obtained at 800~ in air [4.61]. (ii) Influence of dopant and dopant concentration: The ionic conductivity of stabilized Z r O 2 obviously depends on dopant and dopant concentration. Table 4.3 lists the conductivity data for stabilized Z r O 2 doped with various rare-earth oxides.
Chapter 4
80
Z I, fl 100
480
500
520
540
560
580
600
I
i
I
i
I
I
I
80
60 N
|
~o -
~
40 12k
20
/~
2k
I
,r'~
5OO
!
I
I
I
Figure 4.7. Complex impedance plot of polycrystalline (ZrOz)o.9(Y2Oz)o.1 at 800 oC in air [4. 61]
TABLE 4.3
Conductivity Data for Stabilized ZrO 2 Doped with Rare-Earth Oxides [4.35] Dopant (M203)
Nd203 Sm203
Y203 Yb203
Sc203
Composition (mol % M203)
15 10 8 10 10
Conductivity(1000~ (10-2 fl-lcm-l)
Activationenergy (kJ/mol)
1.4 5.8 10.0 11.0 25.0
104 92 96 82 62
With the same dopant concentration, the conductivity of stabilized depends on the size of the dopant cation. Thus, the conductivity increases neodymium to scandium dopant (in the order shown in Table 4.3) since the radius decreases from Nd 3+ to Sc3+. (The radii of Nd 3+, Sm 3+, Gd 3+.
ZrO 2 from ionic y3+,
Yb 3+, and Sc 3§ are 0.104, 0.100, 0.097, 0.092, 0.086, and 0.081 nm, respectively.) One explanation for this trend is that when Zr 4§ (the ionic radius is 0.079 nm) is substituted by a cation with a more similar ionic radius, the
81
Electrolyte
lattice has less strain and fewer association of the cation with oxygen-ion vacancy, e.g., (MzrVo)". This results in greater mobility for oxygen ions, thus higher ionic conductivity. Another explanation for the decrease in conductivity with increasing dopant size is the steric blocking effect of larger cations [4.56, 4.62-4.64]. As seen from Table 4.3, stabilization of ZrO2 with Y203does not yield the highest conductivity. However, Y203-stabilized ZrO2 or YSZ is most frequently used as SOFC electrolyte because of availability and cost. The conductivity of stabilized ZrO2 varies with dopant concentration. Figure 4.8 shows, as an example, variation of conductivity with dopant concentration for various doped ZrO2 compounds at 1080 K [4.42,4.65]. Isothermal plots of conductivity as a function of dopant concentration exhibit a maximum. Above the maximum conductivity dopant concentration, the conductivity decreases with increase in dopant content, and this trend is accompanied by an increase in activation energy for conduction. For the ZrO2Y203 system, the Y203 composition at which the conductivity maximum occurs has not been unambiguously defined, although it appears to fall between 8 and 10 mol % [4.66]. This value is close to or near the minimum quantity of dopant required to fully stabilize the cubic fluorite phase [4.67-4. 76].
10-1
%
102
(,,}
c~
>: I,> Iu a z 0 u
10-3
10-4
l
I
l
I
4
8
12
16
1
2O
MoI% M203 or MO
Figure 4.8. Variation of ionic conductivity of stabilized Z r O 2 with dopant concentration at 1080 K [4.65]
82
Chapter 4
The decrease in conductivity at higher dopant concentrations is believed to be due to defect ordering, vacancy clustering, or electrostatic interaction [4.41]. One such mechanism is discussed here to explain the conductivity behavior of the ZrO2-Y203 system [4.49]. At low Y203 concentrations, the average distance between defect complexes (considered as a one-fold associate defect complex, YZrVo) is large, and each oxygen-ion vacancy is trapped and immobilized inside the defect complex, resulting in low oxygen-ion conductivity. With increasing Y203 concentration, the defect complexes begin to overlap one another. The effective carrier concentration and the migration path for oxygenion vacancies (through these defect complexes) thus increase with accompanying increase in conductivity. Further increase in the Y203concentration leads to the appearance of two-fold associate defect complexes (Y Zr / VOYzr) " / [4. 77]. This decreases the effective carrier concentration and the effective oxygen-ion migration path. The result is a decrease in conductivity, thereby producing a maximum conductivity as a function of dopant concentration. The appearance of a maximum in the oxygen-ion conductivity of stabilized ZrO2 is thus due to increased trapping of vacancies as the concentration of Y203 dopant increases; i.e., as the dopant concentration increases, the distorted region decreases in size, and the disorder becomes dominated by aggregates of clusters. (iii) Influence of temperature: The electrical conductivity of fully stabilized ZrO2 as a function of temperature typically follows Arrhenius-type behavior. Figure 4.9 shows several Arrhenius conductivity plots for YSZ having different Y203contents [4.44]. In general, Arrhenius plots for YSZ tend to show two regions (low-temperature and high-temperature) of different slopes (or conduction activation energies) [4. 78]. The change in the slope of Arrhenius plots has been attributed to the formation of dopant cation/vacancy complexes at low temperatures [4. 79]. The conductivity/temperature relationship for YSZ is given by the following equation [4.80]:
oT
=
Aoexp[-(tz+13T-~r] ~
(Eq. 4.2)
leT where o is the conductivity, T the temperature, r the Boltzmann constant, Ao the preexponential constant, and a and B the positive constants. This equation has been found to hold for both single crystal and polycrystalline YSZ. It should be noted that in a certain temperature range, c~ + BT l can be approximated as constant (thus, giving the activation energy for conduction, E,), and, in this case, the more familiar Arrhenius equation is obtained, i.e., aT = A o exp(-Eo/KT).
Electrolyte
83
I0 s I-
1
1
I
1
I
+
10 tool% Y=,Oz 15 mol%
v//
,
2o.,o1~
/
oo6
l~x
p
///
10 4 -
E U
>2 F-
10 3
/
> ,,=,. I-. 0,.=. '} t,Li
10 2
/
1
0.6
0.7
l
0.8 0.9
lIT,
1
I
l
1.0
1.1
1.2
_
1.3
10"3K "1
Figure 4.9. Arrhenius resistivity plots for Y203-doped ZrO2 materials [4.44]
(iv) Influence of atmosphere: In general, the ionic conductivity of cubic stabilized ZrO2 is independent of oxygen partial pressure over several orders of magnitude (Figure 4.10) [4.81]. Under these conditions, the ionic transport number is very close to unity (i.e., negligible electronic conduction). As discussed in Chapter 3, electronic conductivity in an ionic conductor cannot be absolutely zero. For example, the ionic (ai) and electronic conductivities (ae and oh) of (ZrO2)o.92(Y203)0.08 as a function of temperature (800 ~ to 1050~ and partial pressure of oxygen (0.21 to 10 17 atm or 0.21 x 105 to 10.2 Pa) are given by the following empirical equations [4.82]: o~(~-lcm -1) = 1.63x102exp(
o 9 (~-lcm-l) = 1.31 x
10 7
-0.79 eV ) KT
exp( -3.88 eV) p-1/4o, KT
(Eq. 4.3)
(Eq. 4.4)
84
Chapter 4
lOO
18.18 mol% Y01.5
10-1
33.33 mol% Y01.5 /
15 mol% CaO
/
10-2 46.16 mol% Y01.5
10-3
_
66.67 mol% Y01.5 _
i
10-4 0
I
4
i
I
8
J
1
12
l
l
16
J
I
20
l
1
24
l
2~
-LOG OXYGEN PARTIAL PRESSURE, atm (1.01 x 10 s Pa)
Figure 4.10. Ionic conductivity of stabilized Zr02 at IO00~ as a function Of oxygen partial pressure [4.81]
o h (~-xcm-1) = 2.35 x 102 exp(
- 1.67 e V ) p 114 ~:T o~
(Eq. 4.5)
where eV = 1.6021 • 1 0 -19 J. Under typical SOFC oxygen partial pressures (0.21 to 10 -17 arm), as shown by the equations above, the electronic (electron and hole) conductivities are negligible, compared to the ionic conductivity. At very low oxygen partial pressures, the electronic conductivity then becomes significant, and the total conductivity starts to increase with decreasing oxygen partial pressure (Figure 4.11) [4.83]. The oxygen partial pressure at which the electronic conductivity becomes significant is higher at higher temperatures, as shown in Figure 4.11. In a highly reducing atmosphere, the increase in conductivity occurs mainly in the bulk material. The grain-boundary conductivity varies very little with atmosphere [4.84]. (v) Influence of grain boundary: In SOFCs, YSZ is used in the form of polycrystalline thin films or layers. The conductivity of polycrystalline YSZ is known to consist of the bulk conductivity and the grain-boundary conductivity. The grain-boundary conductivity of stabilized Z r O 2 is mainly due to the presence of impurities or second phases introduced via the raw materials or during
85
Electrolyte
| 700~
800~
900~
~
~:
---
o,/
/
/
700oC
-5
-7 (-.)
/
/ \x
-9
-11
!
0
//,
!,'/ - 10
:\~ ~-""--20
t
-30
!
-40
.
-50
LOG OXYGEN PARTIAL PRESSURE, atm (1.01 x 10 s Pa)
Figure 4.11. Conductivities of (ZrO2)o.9(Y203)o.1 as a function of oxygen partial pressure [4.831
fabrication processes. (In general, grain boundaries are considered as highly disordered regions with possible differences in chemical composition compared to the interior of the grains.) Figure 4.12 shows, as an example, the grainboundary and bulk conductivities of YSZ prepared from two commercial powders [4.851.
Compounds such as SiO2 and AI203 are commonly present as impurities in commercial YSZ powders or added to starting powders as sintering aids. SiO2 and A1203 tend to form thin imergranular glassy phases (composed of SiO2, A1203, and Y203) in YSZ ceramics at high temperatures [4.86-4.88]. These glassy phases tend to be segregated in large isolated pockets along the boundaries [4.89,4.90] or to migrate to the external surface of the ceramics [4.91]. As a result, intergrain (grain-boundary) conductivity is quite different from the intragrain (bulk) conductivity. The grain-boundary conductivity is strongly influenced by several factors such as grain size and impurity level. For small grains (< 2 to 4/~m), grainboundary conductivity is independent of the grain size and is 100 times lower than that of the bulk. For large grains (> 2 to 4 ~tm), grain-boundary conductivity decreases with increasing grain size [4.92-4.94]. The grainboundary conductivity decreases with increased impurity level [4.95,4.96]. In general, for high-density, pure polycrystalline materials, the contribution from
86
Chapter 4 TEMPERATURE, ~ 9 0 0 8 0 0 7 0 0 J6 0 0
500
400
i
i
10-1 ~,,,
GRAIN B O U N D A R Y CONDUCTIVITY
N ~ o ~, ----->r162 . . . . . . r,,.) "7
~,
1 0 -2
POWDER 1 POWDER 2
c
>: I.-> I-C3 :3 a Z 0 fO
10 .3
,o..,
co.ouc.,v,.Y
.
;-, COMM .C,. 10 .4
10
5
owo .,
-'COMMERCIAL POWDER 2
\\\,
9
'
'
,
,
,
,
9
10
11
12
13
14
15
lIT, 104K "1
Figure 4.12. Bulk and grain-boundary conductivities of YSZ samples (preparedfrom two commercial powders) [4.85] the grain-boundary conductivity is relatively small. Also, the influence of grain boundaries is typically considerable at low and intermediate temperatures (e.g., < 700~ At higher temperatures, grain boundaries have a lesser influence on the conductivity, especially when the sample is prepared from powders without the presence of significant amounts of impurities or additives. (v) Influence of time (aging): Stabilized ZrO2 can exhibit a time dependence of its conductivity [4.97-4.99]. This conductivity aging effect has been shown to be especially important in polycrystalline ZrO2 [4.100]. Typically, the bulk conductivity of fully stabilized ZrO2 reaches a steady value in a relatively short time (as shown by measurements of single crystals) [4.80]. This relatively rapid attainment of steady state has been attributed to the reorganization of the crystal [4.100]. The grain-boundary conductivity, on the other hand, tends to change with time. This change mainly involves gradual enhancement of the blocking effect as a result of the segregation of oversaturated impurities at the boundaries [4.100]. For partially stabilized ZrO2, the conductivity aging effect is considered to be due to the precipitation of tetragonal phase from the cubic matrix [4.101].
Electrolyte
87
The time dependence of the resistivity of polycrystalline YSZ has been measured and is given by the following general equation: P(O = A - B x e x p ( - K l t ) - B2exp(-K2t)
(Eq. 4.6)
where o is the resistivity, t the time, and A, B~, K~, B2, and K2 positive constants with the subscripts 1 and 2 designating relations to the bulk and grain-boundary resistances, respectively [4.102]. In SOFC applications where the fully stabilized YSZ electrolyte is typically prepared from pure materials, the conductivity aging effect is often insignificant. 4.2.5 Chemical interaction
At the fuel cell operating temperature (600 ~ to 1000~ stabilized ZrO2 exhibits little or no chemical interaction with other components (LaMnO3 cathode, nickel/YSZ cermet anode, and LaCrO3 interconnect). Chemical interaction of stabilized ZrO2, especially with LaMnO3, becomes more important at higher temperatures (see chemical interaction sections of Chapters 5, 6, and 7 for more details). ZrO2 reacts with LaMnO3 to form insulating phases such as La2Zr207 at the interface at temperatures above 1100 oC [4.103-4.105]. These insulating phases are undesirable in SOFCs and must be minimized because they cause cell performance to degrade significantly. 4.2.6 Thermal expansion
The thermal expansion coefficient of undoped ZrO 2 single crystals is about 8.12 x 10 -6 cm/cm-K in the temperature range of 20 ~ to 1180~ [4.106]. D o p e d Z r O 2 materials typically have higher thermal expansion coefficients. For example, the thermal expansion coefficient of Z r O 2 crystals doped with 4 wt% CaO is about 10.08 x 10 -6 cm/cm.K [4.106]. Table 4.4 lists thermal expansion data for various YzO3-stabilized Z r O 2 materials [4.107]. In general, the thermal expansion of partially stabilized Z r O 2 is very similar to that of fully stabilized material and is essentially unaffected by the presence of tetragonal precipitates [4.106]. The thermal expansion coefficients of Z r O 2 (doped with different Y203 concentrations) at various temperatures are given in Figure 4.13 (from a Tosoh zirconia powder technical bulletin).
Chapter 4
88
TABLE 4.4
Thermal Expansion Data for YzO3-Stabilized ZrO2 Materials
Temperature
Dopant content
(oc)
Thermal expansion coefficient (10.6 cm/cm. K)
Ref.
Single-crystal 5 wt% Y203 8 wt% Y203 12 wt% Y203 20 wt% Y203
20202020-
1500 1500 1500 1500
10.99 10.92 10.23 11.08
[4.106] [4.106] [4.106] [4.106]
Polycrystalline 3 mol% Y203 6 mol % Y203 7.5 mol% Y203 8 mol% Y203 9 mol% Y203
1000 1000 25- 1000 100- 1000 960
10..~ 10.2 10.0 10.8 9.8
[4.108] [4.108] [4.109] [4.110] [4.111]
E (3 =, o
11
==
10 9
z
8
U u
7
U.I
U.
uJ O U Z O
N z <. G x m < W
-r k-
6 9 2mol%Y203
5
4
A
3
0
2
0
3
4
1
2o0
|
,00
i
600
i
1
8o0
i
000
"
"
"
....
9 6
9
"
J
1
200
i
,00
i
600
TEMPERATURE, ~
Figure 4.13. Thermal expansion coefficients of YSZ at different temperatures (from Tosoh Zirconia Powder Technical Bulletin)
89
Electrolyte
As discussed in Chapter 10, a small difference in the thermal expansion coefficients of cell components in the SOFC can produce large stresses during fabrication and operation and cause cracking in the ceramic structure. Therefore, matching thermal expansion in the cell components is critical. Figure 4.14 is an example of thermal expansion curves for several stabilized ZrO2 and perovskite oxide materials to illustrate that without material tailoring or modification, significant thermal expansion mismatch can exist [4.112]. In SOFCs, the YSZ electrolyte is typically selected as the baseline material, and the thermal expansion of other cell materials is modified to match that of the electrolyte. The thermal expansion coefficient of perovskite cathode and interconnect may be adjusted by tailoring the dopant element and concentration (see thermal expansion sections of Chapters 5 and 7). The thermal expansion coefficient of nickel cermet anode may be tailored by modifying the nickel content and ZrO2 concentration or by using additives (see thermal expansion section of Chapter 6).
1
!
o
1.0
g,,.
b
--.
/ / 0.5
a. b. c. d. e. f. g. h.
0.0
. 0
.
.
.
.
(ZrO~lo.91(Sc~O3)o.04slYb~O3)o.04s (ZrO2)o.91(Y203)o.09 Lao.TCao.3 MnOz.~ Lao.TSro.3MnO ~-6 Yo.2Sro..FeO3_ ~ Lao.3Sro.TFeO3. J Ndo.eSro.4CoO3.~ Lao.4Sro.sCoO3.~
L___.
.
.
500
.
! 1000
TEMPERATURE, ~
Figure 4.14. Thermal expansion curves for several stabilized ZrO 2 and perovskite oxide materials [4.112]
90
Chapter 4 4.2.7 Mechanical properties
At room temperature, YSZ (8 mol% Y203) typically has a bending strength of about 300 to 400 MPa and a fracture toughness of about 3 MN-rff/2. The mechanical properties of a YSZ electrolyte layer obviously vary, depending on the characteristics of starting powders used in the fabrication (such as particle size, particle size distribution, and agglomerate strength) and fabrication route and fabrication conditions [4.113-4.117]. For example, YSZ powders having strong and large agglomerates (up to 100/zm in diameter) are difficult to break down and tend to cause defects in the prepared electrolyte, resulting in poor strength of the component [4.114]. YSZ sheets produced by tape calendering have superior mechanical properties, with a mean strength about 15 % higher than that of the material made by tape casting [4.117]. At present, few data have been reported on the mechanical properties of YSZ at elevated temperatures. One measurement indicates a mean strength of about 280 MPa for the YSZ at 900~ as compared to the value of 368 MPa at room temperature [4.117]. A bending strength of about 225 MPa has also been reported for YSZ at 1000~
[4.1181. Using YSZ having high strength and toughness as the electrolyte in SOFCs is desirable. A strong and tough electrolyte is less sensitive to the presence of flaws and imparts better fracture resistance to the fuel cell during fabrication and operation. Several approaches have been taken to improve the mechanical properties of the YSZ. These approaches are based on improvement of fracture resistance of YSZ by toughening. The YSZ has been toughened by introducing inclusions of monoclinic ZrO: [4.119]. However, the addition of monoclinic ZrO2 has been found to cause the conductivity of YSZ to degrade to a level unacceptable for SOFC application. Fine particles of partially stabilized ZrO 2 [4.119], A1203 [4.118,4.120-4.126], and MgO [4.127] have also been added to YSZ. These additives increase the fracture toughness and strength of the YSZ without deleteriously affecting the electrical conductivity of the material. For example, the composition of YSZ with 30 wt% partially stabilized ZrO2 is attractive as the SOFC electrolyte. The fracture toughness of this composition is about 2.95 MPa-rri/2 (200% higher than that of YSZ fabricated under similar process conditions), and the ionic conductivity is about 0.15 fl-~cm-~ (17 % lower than that of YSZ) [4.118]. The composition of YSZ with 20 wt % A1203 has been recommended as the SOFC electrolyte. This composition has a bending strength of 33 kgf/mm 2 or 323 MPa (compared with 24 kgf/mm 2 or 235 MPa for
Electrolyte
91
YSZ) and an ionic conductivity of about O. 10 f}-lcm-1 at 1000~ (compared with 0.12 ~-~cm-~ for YSZ) [4.121]. Figure 4.15 shows an example of the variation of the bending strength of YSZ with temperature and A1203 content [4.118]. Because of high toughness and strength, tetragonal ZrO2 (TZP) has been proposed as a SOFC electrolyte material [4.128-4.131]. For comparison, the toughness of YSZ ranges between 1 and 3 MPa.m--1/2, whereas that of TZP ranges between 6 and 9 MPa.m la At temperatures below 600~ the electrical conductivity of TZP is greater than that of YSZ (Figure 4.16) [4.128,4.129]. This suggests the possibility of its use as electrolyte in SOFCs operated at low temperatures. However, there are two main concerns regarding SOFCs based on TZP electrolyte: mechanical integrity and aging effect. In general, TZP electrolytes can suffer mechanical degradation after long-term exposure to fuel cell operating temperatures. This degradation results from the growth and subsequent transformation of the metastable tetragonal phase [4.132]. This transformation proceeds as a function of time, and the contribution of dislocations and internal stresses is believed to be significant to the tetragonal-to-m0noclinic phase transformation. TZP also shows pronounced conductivity aging [4.133, 4.134]. The aging behavior in TZP is a result, in part, of enhancement of the grain-boundary blocking effect. The segregation of impurities to the grain 40
25oc .
I.(9 z ILl n"
(/3
.
~
30 n
Zm Z'~ ~ Z
20
......../--"~
500~
t...
E ~
Q.
'"'
10
"r I--
1 0
1 10
1 20
1 30
AI20~ CONTENT, wt%
Figure 4.15. Variation of the bend strength of YSZ with temperature and Al20s content [4.]]8]
92
Chapter 4 10 3
i
i
[
f
I
!
i
;
i
-I 10 2
YSZ
v
o
101 i.c o
.,.J
10 0 boundary \
10-~ 1.0
I
! 1.2
.
l
]
,
t
1.4
1/7",
[ 1.6
J
1
_
1.8
103K 1
Figure 4.16. Bulk and grain-boundary conductivities of TZP (bulk conductivity of YSZ includedfor comparison) [4.128]
boundaries during aging is one of the mechanisms responsible for this effect. Furthermore, TZP has been found to have poor phase stability when undergoing thermal cycling between room temperature and 800~ This phase instability results in an increase in monoclinic phase in bulk TZP and at the grain boundary and, accordingly, causes a decrease in both bulk and grain-boundary conductivities [4.135]. Incorporation of CeO2 into TZP appears to reduce the conductivity aging effect [4.136-4.138]. 4.3 DOPED CERIA
Pure C e O 2 has the cubic fluorite structure up to its melting point. Therefore, CeO2, unlike ZrO2, does not need any stabilization. Depending on temperature and oxygen partial pressure, the material exhibits a large oxygen deficiency with the formula CeO2_~, where t5 may be as large as 0.3. For small oxygen deficiencies ((5 < 10-3), doubly ionized oxygen vacancies are the principal ionic defects with compensating electrons [4.139]. For large oxygen deficiencies, a transition toward singly ionized vacancies has been observed. Pure CeO2 has n-type electrical conduction, and the conduction takes place by a smallpolaron hopping mechanism. Pure CeO2 has negligible ionic conductivity. The radius of the Ce 4§ ion in CeO2 is sufficiently large that a variety of dopant can be incorporated to form solid solutions. CeO2 doped with a divalent
Electrolyte
93
or trivalent oxide shows relatively high oxygen-ion conductivity at elevated temperatures. Doped CeO2, however, has the tendency to undergo reduction (Ce 4+ ion to Ce 3+ ion) at low oxygen partial pressures (with the consequent introduction of electronic defects). This reduction restricts the range of oxygen partial pressure over which the ionic transference number remains close to unity. Thus, at 800~ the oxygen partial pressure range for predominant ionic conduction in CeO2 is limited to about 10-~2 atm (10 -7 Pa) [4.56]. Figure 4.17 shows, as an example, the oxygen-ion transference number for La203-doped CeO2 as a function of temperature and dopant content [4.140]. In spite of the tendency to be reduced in a reducing environment, doped CeO2 has been considered for use as SOFC electrolyte, especially at reduced temperatures, because of its high ionic conductivities. Compared to stabilized ZrO2, doped CeO2 shows a higher conductivity and a lower conduction activation energy. Doped CeO2 has also been considered as an electrolyte for SOFCs operated directly on methanol. Various dopants have been used with CeO2, including La203 [4.140, 4.141], Y203 [4.79,4.142-4.148], Sm203 [4.149,4.150], Gd203 [4.148,4.1514.159], other rare-earth oxides [4.160], Gd203+Pr203 [4.161], CaO [4.1454.147, 4.162, 4.163], and SrO [4.164]. The Arrhenius plots for the ionic conductivities of several CeO2 solid solutions are shown in Figure 4.18 [4.165]. Table 4.5 lists conductivity data for various doped CeO2 materials. 1.0 ,,'5,
.,~
CELL
o
-x
.
x
0.9 z
0.8
F,, 0.7
,/
_~ 0.6 X 0.5
0.4
6oooc
/
~176
"
t~
1
0.2
, 1
1
0.3
1
.1
1000~
1
0.4
_1
.
0.5
CONTENT OF LaOl.s, mol
Figure 4.17. Oxygen-iontransference number of La203-doped Ce02 as a function of temperature and dopant content [4.140]
Chapter 4
94
TEMPERATURE, ~ 900 800 700 600
3
I
i
i 0 A
? []
2-
~70
T,
cI
I
e
,.=
i
(CeOJo.e(SmO~.6)o.2 (CeOJo.a(GdO~.s)o.2 (CeOJo.a(YO~.5)o.2 (CeOJo.e(CaO)o.2 9 Ce02 9 (ZrO2)o.es(YO ~.s)o.~5
0
~4o
E
0 "7
500
i-
O El
e
b
II
o
e
0
._I
O l
3-
9
37
II
-I
0.~
i
01
0.8
.
.9
I ,
1.0
!
1.1 1/T, 10"3K"1
l
1
1.2
1.3
1.4
Figure 4.18. Arrhenius plots of ionic conductivities of doped Ce02 compounds [4.165]
TABLE 4.5 Ionic Conductivity of Doped CeO2
Dopant
Content (mol%)
Ionic conductivity at 800~ (10.2 0lcm -1)
Activation energy (kJ/mol)
La203 Y203 Gd203 Sm203 CaO SrO
10 20 20 20 10 10
2.0 5.5 8.3 11.7 3.5 5.0
26 44 49 88 77
Ref.
[4.140] [4.160] [4.160] [4.160] [4.142] [4.164]
95
Electrolyte
For the same dopant concentration, the ionic conductivity of M203-doped CeO 3 (where M is a rare-earth ion) increases with increasing ionic radius (in the order of yttrium, ytterbium, holmium, dysprosium, gadolinium, samarium) to a maximum at a radius of 0.109 nm and then decreases with further increase in ionic radius (in the order of samarium, neodymium, lamhanum) [4.160]. This trend has been attributed to the binding energy between dopant and host cations [4.160, 4.166]. The electrical conductivity of doped CeO2 increases at low oxygen partial pressures (Figure 4.19). This conductivity increase is due to the presence of n-type electronic conduction under those conditions. For SOFC applications, it is important to know the electrolytic and ionic domain boundaries of the electrolyte. The main factors defining the electrolytic and ionic boundaries of doped CeO2 are dopant and temperature. An example of the electrolytic and ionic boundaries as a function of temperature for (CeO2)0.95(Y203)0.05 and (CeO2)0.8(Gd203)0.2 is shown in Figure 4.20 [4.153]. The reduction, thus the electronic conductivity, of doped CeO2 under reducing atmospheres can be minimized by modifying the dopant. A dopant concept has been attempted to improve the ionic domain of CeO2 [4.154]. Certain dopant modifications have been found to improve the ionic boundary to 10-2~ atm (10 -16 Pa) at 700~ For example, the replacement of 3 mol% gadolinium by praseodymium in Ce0.8Gdo.202_ ~ (to form Ce0.8Gdo.lvPr0.0302_a) improves the electrolytic domain of the material by nearly two orders of magnitude without significantly affecting the ionic conductivity [4.161].
|1 10 -0"5 !!
, O A
,
l
i
(CeO2)o.e(SmOl.s)0.2 (CeO2)~176
~___ 10 "1"0
_
(J Z
i0-I.5
~ t
l
I
1
I
1
0
5
10
15
20
-LOG OXYGEN PARTIAL PRESSURE, atm (1.01
x 105Pa)
Figure 4.19. Conductivity of doped CeO2 as a function of oxygen partial pressure [4.160]
96
Chapter 4 t~ I1. m
o
12001000
I-.-
i i--
TEMPERATURE, ~ 800 600 "1
I
!
I
450
400
i
il
I
0
o.
-10
0"5 t.
-20
z
-30 I I
(.9 0
-40
a: (Ce02)o ~s(Y203)o.os b: (CeOz)oi,(Gd203) o.,
!
J
I
,
0.6
0.7
0.8
0.9
I
!
1.0 1.1
!
I
1.2
1.3
_!
1.4 1
..J
1/7", lO'aK "1
Figure 4.20. Electrolytic and ionic domain boundaries of doped CeO2 [4.153]
Another approach to suppress the reduction of CeO 2 under reducing atmospheres is to coat CeO2 solid solutions with a film of a more stable ionic conducting compound. For example, (CeO2)0.8(Sm203)0.2 has been coated with an Y203-stabilized ZrO2 thin layer (e.g., 2/xm thick) on the fuel side to produce a stable SOFC electrolyte [4.160,4.165,4.167-4.170]. In this case, the stability of CeO2 is dependent on the oxygen partial pressure at the ZrO2/CeO2 interface [4.171]. The oxygen partial pressure at the interface, in turn, depends on the transport characteristics, especially the electronic conductivity of CeO2. High electronic conductivity (in addition to high ionic conductivity) of the CeO2 side ensures high oxygen partial pressure at the interface, and, thus, high thermodynamic stability.
4.4 STABILIZED BISMUTHSESQUIOXIDE Pure Bi203 has two crystallographic polymorphs: t5 phase with a fluorite cubic structure above 730~ and ct phase with a monoclinic structure below 730~ di-li203 (having 25 % of the anion sites vacant) exhibits high oxygen-ion conductivity (about 1 fl-lcm-I near the melting point of 825 ~ ot-Bi203 exhibits p-type conduction. The (5 phase of Bi20 a can be stabilized at low temperatures by doping with a certain metal oxide [4.172-4.178].
Electrolyte
97
Among the known oxygen-ion conductors, stabilized Bi203 shows the highest ionic conductivity at comparable temperatures. For example, in certain composition ranges, the conductivities of stabilized Bi203 exceed 10-I ~-lcm-I at 700~ and 10.2 f/-~cm-I at 500~ one to two orders of magnitude higher than that of stabilized ZrO2. This greater ionic conductivity of stabilized Bi203 offers the possibility of its use as electrolyte in SOFCs operated at reduced temperatures. The main drawback of this material is its small oxygen partial pressure range of ionic conduction. Stabilized Bi203 is easily reduced under low oxygen partial pressures and decomposes into bismuth metal at an oxygen partial pressure of about 10-13 atm (10 .8 Pa) at 600~ [4.179]. Therefore, practical use of stabilized Bi203 as SOFC electrolyte requires protection of the material from direct exposure to reducing atmospheres [4.180]. Stabilized Bi203 has a face-centered cubic (fcc) or rhombohedral single phase or both face-centered cubic and rhombohedral phases, depending on the ionic radius of the dopant cation. The fcc phase is obtained when Bi203 is doped with a trivalent, pentavalent, or hexavalent metal oxide, and the ionic radius of the dopant cation is relatively small. The fcc phase is stable over a wide temperature range and shows no phase transformation up to 800~ The rhombohedral phase is obtained when Bi203 is doped with a certain divalent or trivalent metal oxide, and the ionic radius of the dopant cation is relatively large. In this case, at high temperatures, the stabilized material consists of a highconductivity rhombohedral phase,/31. This rhombohedral phase is transformed into another rhombohedral phase,/32, at low temperatures. The rhombohedral phase/32 also exhibits high conductivity, although lower than that of/3~. Both fcc and rhombohedral phases are obtained (depending on composition) when Bi203 is doped with a metal oxide having a metal cation of medium-size ionic radius. Several stabilized Bi203 systems are briefly discussed below. Bi203-MO systems (where M is calcium, strontium, or barium) have been studied. Bi203-MO solid solutions tend to form rhombohedral phase that shows high oxygen-ion conductivity. Figure 4.21 shows the conductivity of Bi203 doped with CaO, SrO, and BaO as a function of temperature [4:172]. These plots exhibit a sharp jump in the conductivity at 600 ~ to 650~ This jump has been attributed to the 131"~132 transition within the rhombohedral structure. Among the various stabilized Bi203 materials, the BaO-dopedBi203 has one of the highest conductivities. For example, at 600~ the conductivity of (BiEO3)0.a4(BaO)0.16 is about 0.88 f/-lcm-I [4.181].
98
Chapter 4 TEMPERATURE, 800
600
1
~
400
'1
1
"I 9 BaO
10 ~
x
SrO 9 CaO
? ~
10 "!
~
10 .2-
0 10"3 --
1 0 .4 0.8
I
1 1.0
1
I
1.2
I
11
1.4
!
1.6
1
1.8
lIT, 10"3K "1
Figure 4.21. Conductivity of Bi203 doped with CaO, SrO, and BaO [4.172] Bi203-M203 systems (where M is a rare-earth metal) have been most extensively studied. In these systems, the range of fcc and rhombohedral phase formation depends on the ionic radius of the rare-earth cation and the rare-earth oxide content (Figure 4.22) [4.182]. Figure 4.23 shows the conductivity of BiEOa-Y203 as a function of dopant concentration and temperature to illustrate the conductivity behavior of BiEOa-M203 systems [4.183]. It can be seen from Figure 4.23 that solid solutions containing more than 25 mol % Y203 show no jump in conductivity over the whole range of temperature examined. The solid solutions having less than 25 mole % Y203, on the other hand, show abrupt increase in conductivity (due to phase transition), and exhibit thermal hysteresis in the Arrhenius plot (as represented by dotted lines in the figure). The minimum dopant content without jump in conductivity corresponds to the lowest content of added oxides for forming the solid solution in the low-temperature
region. Detailed studies on the electronic conductivity of (Bi203)0.73(Y203)0.27 indicate that the lower limit of oxygen partial pressure under which the ionic transference numbers are higher than 0.99 is about 10-13 atm (10 -8 Pa) at 600~ Figure 4.24 shows the oxygen partial pressure dependence of the hole and electron conductivities of Bi203-M203, together with the oxygen-ion conductivity at 500 ~ 600 ~ and 700~ [4.179]. Table 4.6 summarizes the conductivity of various Bi203-M203 materials.
Electrolyte
1 , 2
i
9
99
9
i
-
,,,,
La
E 'Nd Sm Gd
Yb ,
t
A
i
0.5
0.0
x IN
1.0
(gi203)l.x(M203)x
Figure 4.22. Range of face-centered cubic and rhombohedral phase formation of Bi203-M203 systems [4.182] TEMPERATURE, ~ 800
700
600
500
4()0
1
I
I
i
i..
":
100
1 o tool% Y2O3 2 5 mol% 3 20 mol%
.~ :: .
"~ 0..
:
2 i
"*'-,t ~
10 "1
.~3~
510-2
!6
4
25
5 6 7 8
33 mol% 42.5 tool% 50 mol% 60 mol%
mol%
-
~, 3 4
-
g ~
10.3
0.9
1.0
1.1
1.2
1.3
1.4
1.5
1/T, 10-3K1
Figure 4.23. Conductivity of Bi203-Y203 as a function of Y203 concentration and temperature [4.183]
Chapter 4
100
,
,
9
=
..,
at ~, E
,
' 7oo~ 600oc
2
5~176176
1
1"6
-LOG OXYGEN PARTIAL PRESSURE, atm (1.01
• 10 s Pa)
Figure 4.24. Dependence of conductivities of Bi203-M203 on oxygen partial pressure [4.179]
TABLE 4.6
Conductivity Data for
Dopant
Dy203 ErzO3 Y203 Gd203
Nd203 La203
Dopant content (mol % M203)
28.5 20 20 14 10 15
Bi203-M203 Conductivity (10.2 fllcm-1)
500~
700~
0.71 0.23 0.80 0.11 0.30 0.20
14.4 37.0 50.0 12.0 85.0 75.0
Ref.
[4.184] [4.184] [4.183] [4.185] [4.182] [4.182]
Electrolyte
101
Other Bi203-based systems of interest include Bi203-MO2 (M is tellurium; e.g., Bi203-TeO2 [4.186]), Bi203-MO3 (M is tungsten or molybdenum; e.g., Bi203-WO3 [4.187]), Bi203-M205 (M is vanadium, niobium, or tantalum; e.g., Bi203-V205 [4.172,4.188,4.189]), and Bi203-M60~ (M is praseodymium; e.g., Bi203-Pr6Ol~ [4.186]). Bi203 has also been stabilized by two or more oxides. Some examples are Bi203-Y203-Nb205 [4.190], Bi203-Ln2Oa-TeO2 (Ln is lanthanum, samarium, gadolinium, or erbium) [4.191], and Bi4V2_xMxOll_~(M is a divalent to pentavalem cation) (or the so-called BIMEVOX) systems [4.192]. The BIMEVOX systems being investigated include BICUVOX (copper doped), BINIVOX (nickel doped), BIMOVOX (molybdenum doped), BIWVOX (tungsten doped), BIPBVOX (lead doped), BIZNVOV (zinc doped), and BICOVOX (cobalt doped) [4.193-4.196]. 4.5 OTHER OXYGEN-ION CONDUCTORS Pyrochlore oxides (of the general formula A2B207 with a defect fluorite superstructure) have been proposed as SOFC electrolytes. The key features of these materials are their relatively high intrinsic oxygen-ion conductivity (thus no doping is required) and their equilibrium pyrochlore phase (thus no long-term aging effects are expected). Work on pyrochlores has been focused on the (A3+)2(B4+)207 system, especially the Ln2Zr207 where Ln is a lanthanoid such as Gd2(ZrxTil_x)207 (GZT) and Y2(ZrxTil_x)207 (YZT) [4.197-4.202]. Of these pyrochlore compounds, GZT has been suggested as the electrolyte material for SOFCs. When x < 0.2, the compound shows mixed ionic and electronic conduction. However, when x > 0.2, the electronic component of the conductivity decreases markedly. At x > 0.4, the oxygen-ion conductivity dominates and exceeds 10.3.5 91cm -~ at 800~ Increases in ionic conductivity with increasing x in GZT are related to increasing levels of oxygen disorder. The ionic conductivity of the titanate end member, Gd2Ti207, can be increased further by doping, for example, with an acceptor such as calcium on the A site. In general, higher dopant level and closer host/dopant size match lead to high ionic conductivities (with low activation energies) and low electronic conductivities. The GZT system shows a broad ionic domain, e.g., P~ is about 10-21 atm (10 -16Pa) for Gd2(Zro.6Tio.4)207at 1000~ The ionic domain of the material falls rapidly with increasing temperature. Perovskite oxides of the form ABO 3 (A is a divalent or trivalent cation and B is a tetravalent or trivalent cation) have been considered as SOFC
102
Chapter 4
electrolytes, especially for reduced-temperature applications. When substituted with an appropriate dopant, certain perovskite oxides exhibit high ionic conductivity [4.203]. Typically, doped perovskites are pure oxygen-ion conductors at low oxygen partial pressures but become mixed conductors (acquiring p-type electronic conductivity) at high oxygen partial pressures. For example, BaCeO3 doped with 10 mol% gadolinium shows an oxygen-ion conductivity of about 1.1 x 10.2 ~-lcm-I and an electronic conductivity of about 5 x 10.3 f~-lcm-1 in oxygen at 600~ [4.204,4.205]. An empirical approach has been developed to identify perovskite ionic conductors [4.206-4.209]. The approach is based on the relationship between the activation energy for oxygenion conduction and the free volume of lattice structures. The observed trend between the activation and the free volume has been used to develop a free volume maximization algorithm which permits the identification of cations in the perovskite A and B sites to maximize the free volume for ionic transport through the lattice. As an example, some of the perovskites identified are BaCe0.gGdo.~O3, CaAlo.7Tio.303, and SrZr0.9Sc0.103. In ionic-conducting perovskites, the migrating ion may be 02. or H +, depending on the nature of the perovskite and several factors such as water vapor and temperature. For example, the conducting species in DyA103 and BaCeO3 are considered as oxygen ions, whereas in KTaO3, CaHfO3, BaZrO3, and SrCeO3, they are considered as protons. In BaCe0.9Gdo.103_~, the ionic transport mechanism varies with temperature and atmosphere. The conducting species change from protons at temperatures below 600~ to oxygen ions above 900~ under fuel cell operating conditions. Some BaCeO3-based oxides also show mixed oxygen-ion and protonic conduction under SOFC conditions [4.210-4.213]. 4.6 PROTONIC CONDUCTORS
Some perovskite-type materials have been known to exhibit protonic conduction in hydrogen and/or wet atmospheres at high temperatures [4.2144.216]. For example, when A in ABO3 is substituted with an appropriate lowervalency cation, oxygen-ion vacancies are formed to maintain the electroneutrality condition in the crystal. During processing at high temperatures, oxygen-ion vacancies react with oxygen to produce electron holes as shown by the following equation:
10 x. 2 2+ V~176
(Eq. 4.7)
Electrolyte
103
In this case, the material shows r~ixed oxygen-ion and electron hole conduction. However, in a hydrogen atmosphere, electron holes react with hydrogen to produce protons -~I~ + h ' = H §
(Eq. 4.8)
Or, in a wet atmosphere, the following reaction takes place H20 § 2 h ' = ! O 2 + 2 H +
(Eq. 4.9)
or
t-120
•
+
Vo
= Oo
+
2H +
(Eq. 4.10)
or x
1-12o § Oo + V o - 2(OH)o
(Eq. 4.11)
Protons produced in this case (Eqs. 4.9 and 4.10) are considered to be interstitials [4.215,4.217]. On the other hand, hydroxide ions produced (Eq. 4.11) are considered to migrate between sites adjacent to oxygen ions [4.218] or migrate via vacancies [4.204, 4.207]. Hydroxide-ion conduction is considered to occur when water is present in the environment. In doped BaCeO3_~, the activation energy for conduction (typically below 0.52 eV or 50 kJ/mol) is lower than that for the motion of OH-via vacancies (about 0.78 eV or 75 kJ/mol) [4. 218, 4.219], indicating migration of protons as the conduction mechanism. Several proton-conducting perovskites have been studied for use as SOFC electrolytes. The most widely studied high-temperature protonic conductors are the solid solutions based on BaCeO3 and SrCeO 3 [4.220, 4.221]. (i) Doped BaCe03: Doped BaCeO3 has been shown to possess significant proton conduction at high temperatures. For example, BaCe0.85Ca0.~503_~ exhibits a protonic conductivity of about 2 • 10 -3 ~-lcm-1 at 9 0 0 ~ with an activation energy of 0.54 eV (52 kJ/mol) [4.222]. Figure 4.25 shows the structure of BaCe0.9Gd0.102.95 as determined by powder neutron diffraction [4.215,4.223]. The structure is orthorhombic with the lattice constants of a = 0.8773 nm, b = 0.6244 nm, and c = 0.6222 nm. Though this structure does not contain any proton and the chemical formula does not include hydrogen, protonic conduction in the material is possible [4.215]. This is because the compound incorporates water vapor from the atmosphere during preparation and subsequent cooling, and so acquires a concentration of mobile protons. However, under typical SOFC
Chapter 4
104
0
0 2-
cea+(Gd 3"~) 0---
Ba2.+
(....,
a
Figure 4.25. Structure of BaCeo.9Gdo.102.95[4.215]
conditions, doped BaCeO3 may show mixed proton and oxygen-ion conduction. According to Eqs. 4.7 and 4.10, the p-type electronic conductivity of doped BaCeO3 depends on oxygen partial pressure and the protonic conductivity on water vapor pressure as shown by the following equations: (Eq. 4.12) (Eq. 4.13) where K7 and gl0 are the equilibrium constants of Eqs. 4.7 and 4.10, respectively. Figure 4.26 shows the conductivity of BaCe0.gGdo.~O2.95 as a function of oxygen partial pressure at two water vapor pressures [4.215]. According to Eq. 4.13, the protonic conductivity should increase by a factor of 10, since the water partial pressure is increased by a factor of 100. The independence of the conductivity of water vapor partial pressure (as shown in Figure 4.26) suggests that protonic conduction is a minor component in this temperature range. Conductivity measurements for Y203-doped BaCeO 3 treated in H20- and D20saturated gas indicate that the conductivity ratio, tr(H+)/o(D§ is greater than the classical value of ~ and the difference in activation energy is about 0.05 eV (4.8 kJ/mol). Thus, nonclassical proton hopping may occur in doped BaCeO3. The carrier concentration (obtained from analysis of the conductivity preexponential for proton-saturated samples) is nearly an order of magnitude lower than the hydrogen concentration (determined from isotopic exchange), suggesting that a large fraction of protons are in bound sites [4.224].
Electrolyte
105
WATER PARTIAL PRESSURE
TEMPERATURE
2 x 10 .4 atm (OPEN SYMBOLS)
0.25
SYMBOLS)
0.20
o
1200"C 1100*C o 1000*C -, 9 0 O o C o 8000C v
// ~/ /
~- 0.15 >
o
D 0.10 7 o a
o 0 . 0 5 ~ 0.00
=
i
i
25
20
,.
i
i
I
i
15
10
5
0
-LOG OXYGEN PARTIAL PRESSURE, a t m ( 1 . 0 1
l
x 10 s Pa)
Figure 4.26. Conductivity of BaCeo.9Gdo.102.95 as a function of oxygen partial pressure and water partial pressure [4.215] The temperature dependence of the conductivity of BaCel_xMxO3_~ in hydrogen gas is shown in Figure 4.27 [4.225]. As discussed earlier, doped BaCeO3 cam be a proton and oxygen-ion mixed conductors. Some examples are BaCe0.gNdo.lO3_~ [4.226], BaCe0.8Dy0.203_~ [4.212], and BaCel_xSmxO3_~ (x = 0.05 to 0.15) [4.227]. In order to reduce the oxygen-ion contribution to the conductivity, partial substitution of barium with calcium has been suggested. This type of substitution lowers the degree of crystal symmetry and restrains the motion of the oxygen ion [4.228]. Gadolinium-doped BaCeO3 has also been found to exhibit primarily proton conduction. The Gd3+ ions have been suggested as substitutes not only for C e 4+ but also for Ba2+ [4.229-4.331]. (ii) Doped SrCe03: Doped SrCeO3 is another common material being considered as a protonic conductor for SOFC applications. In hydrogen atmospheres, doped SrCeO 3 exhibits significant protonic conductivity. Examples of the conductivities of several doped SrCeO 3 compounds in hydrogen are given in Figure 4.28 [4.232]. The conductivities of SrCel_xMxO3_~ have been determined in a hydrogen atmosphere where M is scandium, zinc, manganese, yttrium, indium, neodymium, samarium, dysprosium, or ytterbium, and x = 0.05 to 0.10 [4.232, 4.233]. The compound SrCe0.95Yb0.0503_~ has a protonic conductivity of 2 x 10 -3 i ] - l c m -l in NE/5% H2 at 600~ with an activation energy of 0.59 eV (57 kJ/mol) [4.234]. The conductivity increases proportionally to the
Chapter 4
106
TEMPERATURE, ~ 1000 900 800 700
10 -1
I
I
I
600
I
I
DOPANT [] Yz03 (x = 0.1)
O Nd203(x = 0.1) A LazOz(x = 0.1) 9Nd203(x = 0.05) V' CaO (x = 0.05)
u "7
>.: 10 .2
"',
t> I-
~....~
E3 z O
%. 10 .3
-
_ _ SrCeo.~gbo.~03.6
O'
7
.8
'
0.9
~
i
1.0
-
i
1.1
1.2
lIT, 103K "1
Figure 4.27. Conductivities of BaCel_~lx03.~ in a hydrogen atmosphere [4.225]
TEMPERATURE, ~ 1000 900
i ~
800
700
i
1
1
~-~ 1 0-2 ~---'~ ~' ~0E
600
i j
1 SrCeossYboosO3.6 2 SrCeo9oYoloO3-6
I ~~~o~3
3 SrCe~176176
1
g ~
10-3
0.8
0.9
1.0
1.1
1.2
1/T, 103K "1
Figure 4.28. Conductivities of doped SrCe03.~ in hydrogen [4.232]
Electrolyte
107
square root of the water vapor pressure (in contrast to BaCeO3) and is independent of the oxygen partial pressure [4.235]. Secondary ion mass spectrometry (SIMS) measurements for SrCe0.95Ybo.05034 indicate protons as the probable conducting species for material annealed both in dry air and in wet hydrogen gas at 800~ [4.236]. Furthermore, the protonic conductivity of SrCeOa-based oxides has been found to increase with increasing content of oxygen-ion vacancy, but it is almost independent of the dopant concentration [4.237]. The activation energy of proton conduction in ytterbium-doped SrCeO 3 is about 0.62 to 0.63 eV (60 to 61 kJ/mol) and independent of dopant coment [4.238-4.240]. The proton concentration in SrCeo.95Ybo.osO34 has been determined to be about 2 mol% at 600~ and 1 mol % at 1000~ in water vapor [4.241, 4.242]. These results appear to support the application of Eq. 4.13 for doped SrCeO3. In addition to doped BaCeO3 and SrCeO3, several other oxides have been investigated as proton-conducting electrolytes for use in SOFCs. Examples of these materials include doped zirconates (CaZrO3, BaZrO3, and SrZrO3) [4.243,4.244], BaTho.9Gdo.~O34 [4.208,4.245], Ba2Gdlnl_xGaxO3 [4.246], and doped KTaO3 [4.247]. To date, work on protonic-conductor SOFCs has been limited to material studies, clarification of the conduction mechanism, and testing of small, laboratory-scale single cells. References
4.1
4.2
4.3 4.4 4.5 4.6
4.7
N.Q. Minh, in Science and Technology of Zirconia V, S.P.S. Badwal, M.J. Bannister, and R.H.J. Hannink (eds.), Technomic Publishing Company, Lancaster, PA, 1993, p. 652. M. Ciftcioglu and M.J. Mayo, paper presented at The Spring Meeting of the Materials Research Society, April 16-21, 1990, San Francisco, CA, Report No. DE90-015700, SAND-90-1639C, CONF-900466-78,National TechnicalInformation Service, Alexandria, VA, 1990. M.A. Janney, C.L. Calhoun, and H.D. Kimrey, J. Am. Ceram. Soc., 75 (1992) 341. S.A. Nightingale, R.H.J. Hannink, and S. Street, see Ref. 4.1, p. 299. C.C. McPheeters and T.D. Claar, in 1986 Fuel Cell Seminar Abstracts, October 2629, 1986, Tucson, AZ, Courtesy Associates, Washington, DC, 1986, p. 64. S.V. Phillips and A.K. Datta, in Proceedings of the Institute of Energy Conference on Ceramics in Energy Applications, April 1990, Sheffield, U.K., Hilger, Bristol, U.K., 1990, p. 183. N.Q. Minh, C.R. Horne, F.S. Liu, D.M. Moffatt, P.R. Staszak, T.L. Stillwagon, and J.J. Van Ackeren, in Proceedings of the 25th IECEC, August 12-17, 1990,
108
4.8
4.9
4.10 4.11
4.12 4.13
4.14 4.15 4.16 4.17 4.18 4.19
4.20 4.21 4.22
4.23 4.24 4.25
Chapter 4
Reno, NV, Vol. 3, American Institute of Chemical Engineers, New York, 1990, p. 230. N.Q. Minh, C.R. Horne, F. Liu, P.R. Staszak, T.L. Stillwagon, and J.J. Van Ackeren, in Proceedings of the First International Symposium on Solid Oxide Fuel Cells, October 16-18, 1989, Hollywood, FL, S.C. Singhal (ed.), Electrochemical Society, Pennington, NJ, 1989, p. 307. N.Q. Minh and C.R. Horne, in Proceedings of the 14th Riso International Symposium on Materials Science, High Ten~erature Electrochemical Behaviour of Fast Ion and Mixed Conductors, September 6-10, 1993, Roskilde, Denmark, F.W. Poulsen, J.J. Bentzen, T. Jacobsen, E. Skou, and M.J.L. OstergArd (eds.), Riso National Laboratory, Roskilde, Denmark, 1993, p. 337. A.O. Isenberg, Solid State lonics, 3/4 (1981) 431. Y. Ohno, S. Nagata, and H. Sato, in Proceedings of the 15th IECEC, August 18-22, 1980, Seattle, WA, American Institute of Aeronautics and Astronautics, New York, 1980, p. 881. M.F. Carolan and J.N. Michaels, Solid State Ionics, 25 (1987) 207. N. Nakagawa, C. Kuroda and M. Ishida, in Proceedings of the International Symposium on Solid Oxide Fuel Cells, November 13-14, 1989, Nagoya, Japan, O. Yamamoto, M. Dokiya, and H. Tagawa (eds.), Science House, Tokyo, Japan, 1989, p. 58. H. Arai, see Ref. 4.13, p. 12. T. Setoguchi, M. Sawano, E. Eguchi, and H. Arai, Solid State Ionics, 40/41 (1990) 502. Z. Ogumi, Y. Tsuji, Y. Uchimoto, and Z. Takehara, see Ref. 4.13, p. 203. N. Nakagawa, S. Kosuge, H. Tsuneizumi, E. Matsuda, H. Mihara and Y. Sato, see Ref. 4.8, p. 71. K. Tsukamoto, F. Uchiyama, Y. Kaga, Y. Ohno, T. Yanagisawa, A. Monma, Y. Takahagi, M. J. Lain, and T. Nakajima, Solid State Ionics, 40/41 (1990) 1003. N. Nicoloso, B. Leibold, and H.U. Habermeier, in Laser Ablation of Electronic Materials, E. Fogarassy and S. Lazare (eds.), Elsevier, Amsterdam, The Netherlands, 1992, p. 385. T.W. Kueper, S.J. Visco, and L.C. DeJonghe, Solid State lonics, 52 (1992) 251. E.-T. Kim, J.W. Lee and S.-G. Yoon, J. Electrochem. Soc., 140 (1993) 2625. B.L. Halpern, J.J. Schmitt, J.W. Golz, and Y. Di, in Proceedings of the Fourth Annual Fuel Cell Contractors Review Meeting, July 14-15, 1992, Morgantown, WV, W.J. Huber (ed.), Report No. DOE/METC-92/6127, U.S. Department of Energy, Washington, DC, 1992, p. 102. T. Ishihara, K. Sato, Y. Mizuhara, and Y. Takita, Chem. Lett., (1992)943. T. Namikawa, Y. Yamazaki, I. Saitoh, T. Kanai, S. Sumiya, and M. Satoh, Denki Kagaku, 52 (1984) 714. H. Hamatani, T. Okada, and T. Yoshida, see Ref. 4.13, p. 197.
Electrolyte
4.26 4.27
4.28 4.29 4.30 4.31 4.32 4.33 4.34 4.35 4.36 4.37 4.38 4.39 4.40 4.41 4.42
4.43 4.44 4.45 4.46 4.47 4.48
4.49
4.50 4.51
109
R.T. Brook, in Science and Technology of Zirconia, A.H. Heuer and L.W. Hobbs (eds.), American Ceramic Society, Columbus, OH, 1981, p. 272. M.A.C.G. van de Graaf and A.J. Burggraaf, in Science and Technology of Zirconia //, N. Claussen, M. Riihle, and A.H. Heuer (eds.), American Ceramic Society, Columbus, OH, 1984, p. 744. C.E. Scott and J.S. Reed, Am. Ceram. Soc. Bull., 57 (1978) 741. C.E. Scott and J.S. Reed, Am. Ceram. Soc. Bull., 58 (1979) 587. Science and Technology ofZirconia, A.H. Heuer and L.W. Hobbs (eds.), American Ceramic Society, Columbus, OH, 1981. Science and Technology of Zirconia H, N. Claussen, M. RiJhle, and A.H. Heuer (eds.), American Ceramic Society, Columbus, OH, 1984. Science and Technology of Zirconia III, S. Somiya, N. Yamamoto, and H. Yanagida (eds.), American Ceramic Society, Westerville, OH, 1988. Science and Technology of Zirconia V, S.P.S. Badwal, M.J. Bannister, and R.H.J. Hannink (eds.), Technomic Publishing Company, Lancaster, PA, 1993. R. Stevens, An Introduction to Zirconia, Magnesium Elektron, London, U.K., 1986. T.H. Etsell and S.N. Flengas, Chem. Rev., 70 (1970) 339. E.C. Subbarao and H.S. Maiti, Solid State Ionics, 11 (1984) 317. V.S. Stubican and J.R. Hellmann, see Ref. 4.26, p. 25. V.S. Stubican, see Ref. 4.32, p. 71. H.G. Scott, J. Mater. Sci., 10 (1975) 1527. R.A. Miller, J.L. Smialek, and R.G. Garlick, see Ref. 4.26, p. 241. Y. Suzuki and T. Takahashi, J. Chem. Soc. Jpn, (1977) 1610. H. Tannenberger, H. Schachner, and P. Kovacs, in Proceedings of JournOes Internationales d'Etude des Piles ?t Combustible III, June 21-24, 1965, Soci6t6 d'Etudes de Recherches et d'Application pour l'Industrie, Brussels, Belgium, 1965, p. 19. D.W. Stickler and W.G. Carlson, J. Am. Ceram. Soc., 48 (1965) 286. J.M. Dixon, L.D. LaGrange, U. Merten, C.F. Miller, and J.P. Porter, II, J. Electrochem. Soc., 110 (1963) 276. S.P.S. Badwal and J. Drennan, Solid State Ionics, 53-56 (1992) 769. T. Ishii, T. Iwata, Y. Tajima, and A. Yamaji, Solid State Ionics, 57 (1992) 153. S.P.S. Badwal, J. Mater. Sci., 22 (1987) 4125. K.J. de Vries, T. van Dijk, and A.J. Burggraaf, in Fast Ion Transport in Solids, P. Vashishta, J.M. Mundy, and G.K. Shenoy (eds.), North Holland, New York, 1979, p. 679. N.H. Andersen, K. Claussen, M.A. Hackett, W. Hayes, M.T. Hutchings, J.E. Macdonald, and R. Osborn, in Transport-Structure Relations in Fast Ion and Mixed Conductors, F.W. Poulsen, N.H. Andersen, K. Clausen, S. Skaarup, and O.T. Sorensen (eds.), Riso National Laboratory, Roskilde, Denmark, 1985, p. 279. M. Guillow, Rev. General Elect., 76 (1967) 58. M. Goge, G. Letisse, and M. Gouet, see Ref. 4.27, p. 584.
110
4.52 4.53 4.54 4.55
4.56 4.57
4.58 4.59 4.60 4.61 4.62
4.63 4.64 4.65 4.66
4.67 4.68 4.69 4.70
4.71 4.72 4.73 4.74 4.75 4.76 4.77 4.78
Chapter 4
R.E.W. Casselton, J. Appl. Electrochem., 4 (1974) 25. M. Kleitz, M. Levy, J. Fouletier, and P. Farby, see Ref. 4.26, p. 337. Y. Suzuki and T. Takahashi, Denki Kagaku, 39 (1971) 406. S.P.S. Badwal, in Proceedings of the International Seminar on Solid State Ionic Devices, July 18-23, 1988, Singapore, B.V.R. Chowdari and S. Radhakrishna (eds.), World Scientific, Singapore, 1988, p. 165. B.C.H. Steele, in High Conductivity Solid Ionic Conductors, Recent Trends and Applications, T. Takahashi (ed.), World Scientific, Singapore, 1989, p. 402. N. Bonanos, B.C.H. Steele, E.P. Butler, W.B. Johnson, W.L. Worrell, D.D. Macdonald, and M.C.H. McKubre, in Impedance Spectroscopy, J.R. Macdonald (ed.), Wiley-Interscience, New York, 1987, p. 191. E.P. Butler, R.K. Slotwinski, N. Bonanos, J. Drennan, and B.C.H. Steele, see Ref. 4.27, p. 572. J.E. Bauerle, J. Phys. Chem. Solids, 30 (1969) 2657. E.J.L. Schouler, Ph. D. Thesis, Institut National Polytechnique de Grenoble, Grenoble, France, 1979. T. Takahashi, H. Iwahara, and Y. Suzuki, Denki Kagaku, 39 (1971) 665. J.A. Kilner and J.D. Faktor, in Progress in Solid Electrolytes, T.W. Wheat, A. Ahmad, and A.K. Kuriakose (eds.), Department of Energy, Mines, and Resources, Ottawa, Canada, 1983, p. 347. R.J. Stufford, S.J. Rothman, and J.L. Routbort, Solid State lonics, 37 (1989) 67. S.P.S. Badwal, Solid State Ionics, 52 (1992) 23. J.F. Baumard and P. Abelard, see Ref. 4.27, p. 555. T. Takahashi and Y. Suzuki, in Proceedings of Deuxiemes Journ~es Internationales d'Etude des Piles ~ Combustible, June 19-23, 1967, Soci6t6 d'Etudes de Recherches et d'Application pour l'Industrie, Soci6t6 Commerciale d'Applications Scientifiques, Brussels, Belgium, 1967, p. 378. V.S. Stubican, R. C. Hink, and S.P. Ray, J. Am. Ceram. Soc., 61 (1978) 17. C. Pascual and P. Duran, J. Am. Ceram. Soc., 66 (1983) 23. V.S. Stubican, G.S. Corman, J.R. Hellmann, and G. Senti, see Ref. 4.27, p. 96. T. Sakuma and H. Hata, in Zirconia '88, Advances in Zirconia Science and Technology, S. Meriani and C. Palmonari (eds.), Elsevier, Barking, Essex, U.K., 1989, p. 283. V. Lanteri, A.H. Heuer, and T.E. Mitchell, see Ref. 4.27, p. 118. M. Riihle, N. Claussen, and A.H. Heuer, see Ref. 4.27, p. 352. N. Yoshikawa, H. Eda, and H. Suto, J. Jpn. Inst. Met., 50 (1986) 113. R. Chaim, M. R0hle, and A.H. Heuer, J. Am. Ceram. Soc., 68 (1985) 427. R. Ruh, K.S. Mazdiyasni, P.G. Valentine, and H.O. Bielstein, J. Am. Ceram. Soc., 67 (1984) C-190. Y. Suzuki and T. Takahashi, J. Chem. Soc. Jpn., (1977) 1610. A. Nakamura and J.B. Wagner, Jr., J. Electrochem. Soc., 133 (1986) 1542. S.P.S. Badwal and M.V. Swain, J. Mater. Sci. Lett., 4 (1985) 487.
Electrolyte
4.79 4.80 4.81 4.82 4.83 4.84 4.85 4.86 4.87 4.88 4.89 4.90 4.91
4.92 4.93 4.94 4.95 4.96 4.97 4.98 4.99 4.100 4.101 4.102 4.103 4.104
4.105 4.106
111
D.Y. Wang, D.S. Park, J. Griffith, and A.S. Nowick, Solid State Ionics, 2 (1981) 95. Y. Suzuki and K. Sugiyama, J. Ceram. Soc. Jpn. Intl. Ed., 95 (1987) 480. E.C. Subbarao, see Ref. 4.26, p. 1. J.H. Park and R.N. Blumenthal, J. Electrochem. Soc., 136 (1989) 2867. W. Weppner, J. Solid State Chem., 20 (1977) 305. A. Ovenston, Solid State lonics, 58 (1992) 221. B.C.H. Steele, J. Drennan, R.K. Slotwinski, N. Bonanos, and E.P. Butler, see Ref. 4.26, p. 286. M.L. Mecartney, J. Am. Ceram. Soc., 70 (1987) 54. D.R. Clark, J. Am. Ceram. Soc., 70 (1987) 15. T. Sato, M. Nauer, and C. Carry, J. Am. Ceram. Soc., 74 (1991) 2615. S.P.S. Badwal and J. Drennan, J. Mater. Sci., 22 (1987) 3231. S.P.S. Badwal and J. Drennan, Mater. Forum, 10 (1987) 197. S.P.S. Badwal and A.E. Hughes, in Proceedings of the Second International Symposium on Solid Oxide Fuel Cells, F. Grosz, P. Zegers, S.C. Singhal, and O. Yamamoto (eds.), Commission of The European Communities, Luxembourg, 1991, p. 445. M.J. Verkerk, B.J. Middelhuis and A.J. Burggraaf, Solid State lonics, 6 (1982) 159. S.P.S. Badwal, Appl. Phys. A, 50 (1990) 449. A. Orliukas, P. Bohac, K. Sasaki, M. G6dickemeier, and L.J. Gauckler, see Ref. 4.9, p. 363. M.V. Inozemtsev and M.V. Perfil'ev, Elektrokhimiya, 11 (1975) 1031. M.J. Verkerk, A.J.A. Winnubst, and A.J. Burggraaf, J. Mater. Sci., 17 (1982) 3113o T. Takahashi and Y. Suzuki, Denki Kagaku, 34 (1966) 887. W. Baukal, Electrochim. Acta, 14 (1969) 1071. W. Baukal, in From Electrocatalysis to Fuel Cells, G. Sandstede (ed.), University of Washington Press, Seattle, WA, 1972, p. 247. M. Kleitz, H. Bernard, E. Fernandez, and E. Schouler, see Ref. 4.26, p. 310. F.K. Moghadam and D.A. Stevenson, J. Am. Ceram. Soc., 65 (1982) 213. Y. Suzuki, A. Shimada, and S. Senda, Solid State Ionics, 42 (1990) 121. J.A.M. van Roosmalen and E.H.P. Cordfunke, Solid State lonics, 52 (1992) 303. C.C. Chen, M.M. Nasrallah, and H.U. Anderson, in Proceedings of the Third International Symposium on Solid Oxide Fuel Cells, May 16-22, 1993, Honolulu, HI, S.C. Singhal and H. Iwahara (eds.), ElectrochemicalSociety, Pennington, NJ, 1993, p. 598. C. Clausen, C. Bagger, J.B. Bilde-Sorensen, and A. Horsewell, Solid State lonics, 70/71 (1994) 59. J.W. Adams, H.H. Nakamura, R.P. Ingel, and R.W. Rice, J. Am. Ceram. Soc., 68 (1985) C-228.
112
4.107 4.108 4.109 4.110 4.111 4.112
4.113 4.114 4.115 4.116
4.117 4.118 4.119
4.120 4.121 4.122 4.123 4.124 4.125 4.126 4.127 4.128 4.129 4.130 4.131 4.132 4.133 4.134 4.135 4.136
Chapter 4
J. Gerretsen, A. Mackor, J.P.G.M. van Eijk, and T.P.M. Koster, see Ref. 4.91, p. 159. Tosoh Zirconia Powder Technical Bulletin, Tosoh Corporation, Tokyo, Japan. M. Mori, H. Itoh, N. Mori, T. Abe, O. Yamamoto, Y. Takeda, and N. Imanishi, see Ref. 4.1, p. 776. R. M/inner, E. Ivers-Tiff6e, and W. Wersing, see Ref. 4.91, p. 715. A. Hammouche, E. Siebert, and A. Hammou, Mater. Res. Bull., 24 (1989) 367. T. Takahashi and Y. Suzuki, in Technical Research on the Effective Use of Energy Report, Special Project Research Under Grant in Aid of Scientific Research, Ministry of Education, Tokyo, Japan, 1980, p. 319. B.C.H. Steele, see Ref. 4.13, p. 135. K. Kendall, see Ref. 4.91, p. 429. H. Greiner, E. Keim, W. Kleinlein, and E. Weil~, see Ref. 4.91, p. 705. B.C.H. Steele, C.A. Leach, R.A. Rudkin, N. Khan, and M.H. Huang, in 1990 Fuel Cell Seminar Abstracts, November 25-28, 1990, Phoenix, AZ, Courtesy Associates, Washington, DC, 1990, p. 123. B.C.H. Steele, see Ref. 4.1, p. 713. O. Yamamoto, Y. Takeda, N. Imanishi, T. Kawahara, G. Q. Shen, M. Mori, and T. Abe, see Ref. 4.91, p. 437. J.P. Singh, A.L. Bosak, D.W. Dees, and C.C. McPheeters, in 1988 Fuel Cell Seminar Abstracts, October 23-26, 1988, Long Beach, CA, Courtesy Associates, Washington, DC, 1988, p. 145. F. Ishizaki, T. Yoshida, and S. Sakurada, see Ref. 4.8, p. 3. F. Ishizaki, T. Yoshida, and S. Sakurada, see Ref. 4.13, p. 172. M.T. Hern~indez, J.R. Jurado, and P. Dur~in, see Ref. 4.91, p. 412. O. Yamamoto, T. Kawahara, Y. Takeda, N. Imanishi, and Y. Sakaki, see Ref. 4.1, p. 733. M.I. Osendi and J.R. Jurado, see Ref. 4.104, p. 82. W. Sch/ifer, H. Geier, G. Lindemann, and D. Stolten, see Ref. 4.9, p. 409. M. Sumi, K. Mori, N. Uchida, and K. Uematsu, see Ref. 4.9, p. 431. P. Dur~in, J.R. Jurado, C. Moure, M.T. Hern~indez, and F. Capel, see Ref. 4.91, p. 401. W. Weppner, see Ref. 4.13, p. 83. W. Weppner and H. Schubert, see Ref. 4.32, p. 837. W. Weppner, Solid State Ionics, 52 (1992) 15. Q.H. Gao, R.E. Rocheleau, and B.Y. Liaw, see Ref. 4.104, p. 38. T. Sato and M. Shimada, J. Am. Ceram. Soc., 67 (1984)C-212. A.N. Vlasov and M.V. Perfiliev, Solid State Ionics, 25 (1987) 245. A. E1 Barhmi, E.J.L. Schouler, A. Hammou, and M. Kleitz, see Ref. 4.32, p. 885. T.L. Wen, Z.Y. Lu, and S.F. Li, Solid State Ionics, 28-30 (1988) 475. M.T. Hern~indez, J.R. Jurado, andP. Dur~in, Solid State lonics, 51 (1992) 147.
Electrolyte
4.137
4.138 4.139 4.140 4.141 4.142 4.143 4.144 4.145 4.146 4.147 4.148 4.149 4.150
4.151 4.152 4.153
4.154 4.155 4.156 4.157 4.158 4.159 4.160 4.161 4.162 4.163 4.164 4.165
113
P. Dur~in, M.T. Fern~indez, C. Moure, M. Gonzalez, P. Recio, C. Pascual, and R. Jurado, in Ceramic Today - Tomorrow's Ceramics, P. Vincenzini (ed.), Elsevier, Amsterdam, The Netherlands, 1991, p. 2219. M.T. Fern~indez, J.R. Jurado, P. Dur~in, J.C.C. Abrantes, and F.M.B. Marques, Solid State Ionics, 50 (1992) 167. H.L. Tuller and A.S. Nowick, J. Electrochem. Soc., 126 (1979) 209. T. Takahashi, K. Ito, and H. Iwahara, see Ref. 4.42, p. 42. T. Takahashi and H. Iwahara, Denki Kagaku, 34 (1966) 254. H.L. Tuller and A.S. Nowick, J. Electrochem. Soc., 122 (1975) 255. P. Sarkar and P.S. Nicholson, Solid State lonics, 21 (1986) 49. C. Wang, X. Xu, and B. Li, Solid State Ionics, 13 (1984) 135. A.S. Nowick, D.Y. Wang, D.S. Park, and J. Griffith, see Ref. 4.48, p. 673. D.Y. Wang and A.S. Nowick, Solid State Ionics, 5 (1981) 551. D.Y. Wang and A.S. Nowick, J. Solid State Chem., 35 (1980) 325. R.G. Anderson and A.S. Nowick, in Transport in Non-Stoichiometric Compounds, G. Sinkovich (ed.), Plenum Press, New York, 1985, p. 111. H. Yahiro, Y. Eguchi, K. Eguchi, and H. Arai, J. Appl. Electrochem., 18 (1988) 527. D. Petersen and J. Winnick, in Proceedings of the 28th IECEC, August 8-13, 1993, Atlanta, GA, Vol. 1, American Chemical Society, Washington, DC, 1993, p. 1.1249. T. Kudo and H. Obayashi, J. Electrochem. Soc., 122 (1975) 142. T. Kudo and H. Obayashi, J. Electrochem. Soc., 123 (1976) 415. H. Obayashi and T. Kudo, in Solid State Chemistry of Energy Conversion and Storage, J.B. Goodenough and M.S. Whittingham (eds.), American Chemical Society, Washington, DC, 1977, p. 316. T.E. Swarr, S. Karavolis, and D.L. Maricle, see Ref. 4.7, p. 256. B. Zachau-Christiansen, T. Jacobsen, K. West, and S. Skaarup, see Ref. 4.104, p. 104. S. E1-Houte and M.E.S. Ali, Ceram. Int., 13 (1987)p.243. T. Ivers-Tiff6e and D. Kiistner, Silic. Ind., 49 (1984) 227. I. Riess, D. Braunshtein, and D.S. Tannhauser, J. Am. Ceram. Soc., 64 (1981) 479. R.G. Anderson and A.S. Nowick, Solid State lonics, 5 (1981) 547. H. Yahiro, E. Eguchi, and H. Arai, Solid State lonics, 36 (1989) 71. D.L. Maricle, T.E. Swarr, and S. Karavolis, Solid State lonics, 52 (1992) 173. H. Arai, T. Kunisaka, Y. Shimizu, and T. Seiyama, Solid State lonics, 20 (1986) 241. R.N. Blumenthal, F.S. Brugner, and J.E. Garnier, J. Electrochem. Soc., 120 (1973) 1230. H. Yahiro, K. Eguchi, and H. Arai, Solid State lonics, 21 (1986) 37. K. Eguchi, T. Setoguchi, T. Inoue, and H. Arai, Solid State Ionics, 52 (1992) 165.
114
4.166 4.167 4.168 4.169 4.170 4.171 4.172 4.173 4.174
4.175 4.176 4.177 4.178 4.179 4.180 4.181 4.182 4.183 4.184 4.185 4.186 4.187 4.188 4.189 4.190 4.191 4.192 4.193
Chapter 4
V. Butler, C.R.A. Catlow, B.E.F. Fender, and J.H. Harding, Solid State Ionics, 8 (1983) 109. H. Yahiro, Y. Baba, K. Eguchi, and H. Arai, J. Electrochem. Soc., 135 (1988) 2077. T. Inoue, T. Setoguchi, K. Eguchi, and H. Arai, Solid State lonics, 35 (1989) 285. H. Arai, K. Eguchi, T. Setoguchi, H. Itoh, and T. Inoue, see Ref. 4.8, p. 288. K. Mehta, S.J. Hong, J.-F. Jue, and A.V. Virkar, see Ref. 4.104, p. 92. A.V. Virkar, J. Electrochem. Soc., 138 (1991) 1481. T. Takahashi and H. Iwahara, Mater. Res. Bull., 13 (1978) 1447. T. Takahashi, in Superionic Solids and Solid Electrolytes, Recent Trends, A.L. Laskar and S. Chandra (eds.), Academic Press, San Diego, CA, 1989, p. 1. H.D. Baek and A.V. Virkar, in Proceedings of the First International Symposium on Ionic and Mixed Conducting Ceramics, October 16-17, 1991, Phoenix, AZ, T.A. Ramanarayanan and H.L. Tuller (eds.), Electrochemical Society, Pennington, NJ, 1991, p. 57. T. Suzuki, T. Yamazaki, K. Kaku, and M. Ikegami, Solid State lonics, 15 (1985) 241. J.C. Boivin and D.J. Thomas, Solid State lonics, 3/4 (1981) 457. J.C. Boivin and D.J. Thomas, Solid State lonics, 5 1981) 523. J.A. Kilner, J. Drennan, P. Dennis, and B.C.H. Steele, Solid State lonics, 5 (1981) 527. T. Takahashi, T. Esaka, and H. Iwahara, J. Appl. Electrochem., 7 (1977) 303. A.M. Azad, S. Larose, and S.A. Akbar, J. Mater. Sci., 29 (1994) 4135. T. Suzuki, Y. Dansui, T. Shirai, and C. Tsubaki, J. Mater. Sci., 20 (1985) 3125. H. Iwahara, T. Esaka, T. Sato, and T. Takahashi, J. Solid State Chem., 39 (1981) 173. T. Takahashi, H. Iwahara, and T. Arao, J. Appl. Electrochem., 5 (1975) 187. M.J. Verkerk and A.J. Burggraaf, J. Electrochem. Soc., 128 (1981) 75. P. Su and A.V. Virkar, J. Electrochem. Soc., 139 (1992) 1671. T. Esaka, T. Mangahara, and H. Iwahara, Solid State lonics, 36 (1989) 129. T. Takahashi and H. Iwahara, J. Appl. Electrochem., 3 (1973) 65. T. Takahashi, H. Iwahara, and T. Esaka, J. Electrochem. Soc., 124 (1977) 1563. F. Abraham, M.F. Debreulle-Gresse, G. Mairesse, and G. Nowogrocki, Solid State lonics; 28-30 (1988) 529. G. Meng, C. Chen, X. Han, P. Yang, and D. Peng, Solid State lonics, 28-30 (1988) 533. D. Mercurio, M. E1 Farissi, B. Frit, J.M. Reau, and T. Senegas, Solid State lonics, 39 (1990) 279. J.B. Goodenough, A. Manthiram, H. Paranthaman, and Y.S. Zhen, Solid State lonics, 52 (1992) 105. T. Iharada, A. Hammouche, J. Fouletier, M. Kleitz, J.C. Boivin, and G. Mairesse, Solid State lonics, 48 (1991) 257.
Electrolyte
4.194 4.195
4.196
4.197 4.198 4.199 4.200 4.201 4.202 4.203 4.204 4.205 4.206 4.207 4.208 4.209 4.210 4.211 4.212 4.213 4.214 4.215 4.216 4.217 4.218 4.219 4.220 4.221 4.222
115
J.C. Boivin, R.N. Vannier, G. Mairesse, F. Abraham, and G. Nowogrocki, ISSI Lett., 3 (1992) 14. P. Strobel, E. Pemot, M. Bacmann, J. Fouletier, T. Iharada, G. Mairesse, and F. Abraham, in Proceedings of Symposium A2 on Solid State Ionics, International Conference on Advanced Materials- ICAM91, May 27-31, 1991, Strasbourg, France, M. Balkanski, T. Takahashi, and H.L. Tuller (eds.), North Holland, Amsterdam, The Netherlands, 1992, p. 387. G. Mairesse, in Fast Ion Transport in Solids, NATO Advanced Science Institute Series E: Applied Science, Vol. 250, B. Scrosati, A. Magistris, C.M. Mari, and G. Mariotto (eds.), Kluwer Academic, Dordrecht, The Netherlands, 1993, p. 271. A.J. Burggraaf, T. van Dijk, and M.J. Verkerk, Solid State lonics, 5 (1981) 519. P. K. Moon and H.L. Tuller, see Ref. 4.8, p. 30. M. Spears, S. Kramer, H.L. Tuller, and P.K. Moon, see Ref. 4.174, p. 32. H.L. Tuller and P.K. Moon, Mater. Sci. Eng., B1 (1988) 171. H.L. Tuller, S. Kramer, and M.A. Spears, see Ref. 4.9, p. 151. S.Kramer, M. Spears, and H.L. Tuller, see Ref. 4.104, p. 119. T. Takahashi and H. Iwahara, Energy Convers., 11 (1971) 105. N. Bonanos, B. Ellis, K.S. Knight, and M.N. Mahmood, Solid State Ionics, 35 (1989) 179. N. Bonanos, B. Ellis, and M.N. Mahmood, Solid State Ionics, 44 (1991) 305. R.L. Cook, R.C. MacDuff, and A.F. Sammells, J. Electrochem. Soc., 137 (1990) 3309. R.L. Cook and A.F. Sammells, Solid State lonics, 45 (1991) 311. A.F. Sammells, R.L. Cook, J.H. White, J.J. Osborne, and R. C. MacDuff, Solid State Ionics, 52 (1992) 111. K. Krist, R.L. Cook, and A.F. Sammells, see Ref. 4.91, p. 237. T. Yajima, H. Iwahara, and H. Uchida, Solid State Ionics, 47 (1991) 117. H. Iwahara, Solid State Ionics, 52 (1992) 99. H. Iwahara, T. Hibino and M. Yamada, see Ref. 4.104, p. 137. N. Taniguchi, K. Hatoh, J. Niikura, T. Gamo, and H. Iwahara, Solid State Ionics, 53-56 (1992) 998. T. Takahashi and H. Iwahara, Rev. Chim. Min~r., 17 (1980) 243. N. Bonanos, Solid State Ionics, 53-56 (1992) 967. T. Norby, Solid State Ionics, 40/41 (1990) 857. S. Shin, H.H. Huang, M. Ishigame, and H. Iwahara, Solid State lonics, 40/41 (1990) 910. R.T.C. Slade and N. Singh, Solid State Ionics, 46 (1991) 111. R.T.C. Slade and N. Singh, Solid State Ionics, 61 (1993) 111. N. Bonanos, see Ref. 4.9, p. 19. J.R. Jewulski, T.L. Osif, and R.J. Remick, Solid-State Proton Conductors, U.S. Department of Energy, Report No. DOE/MC/24218-2957, Washington, DC, 1990. R.C.T. Slade, S.D. Flint, and N. Singh, see Ref. 4.9, p. 417.
116
4.223 4.224 4.225 4.226 4.227 4.228 4.229 4.230 4.231
4.232 4.233 4.234 4.235 4.236 4.237 4.238 4.239 4.240 4.241 4.242 4.243 4.244 4.245 4.246 4.247
Chapter 4
K.S. Knight, M. Soar, and N. Bonanos, J. Mater. Chem., 2 (1992) 709. T. Scherben, Yu.M. Baikov, and E.K. Shalkova, Solid State Ionics, 66 (1993) 159. H. Iwahara, H. Uchida, K. Ono, and K. Ogaki, J. Electrochem. Soc., 135 (1988) 529. H. Iwahara, H. Uchida, and K. Morimoto, J. Electrochem. Soc., 137 (1990)462. H. Iwahara, T. Yajima, T. Hibino, and H. Uchida, J. Electrochem. Soc., 140 (1993) 1687. T. Yajima, H. Iwahara, and H. Uchida, Solid State Ionics, 47 (1991) 117. K.D. Kreuer, E. Sch6nherr, and J. Maier, see Ref. 4.9, p. 297. H. Iwahara, T. Yajima, T. Hibino, K. Ozaki, and H. Suzuki, Solid State lonics, 61 (1993) 65. J.F. Liu and A.S. Nowick, in MRS Syn~osium Proceedings, Solid State Ionics, Vol. 210, G.A. Nazri, D.F. Shriver, R.A. Huggins, and M. Balkanski (eds.), Material Research Society, Pittsburgh, PA, 1991, p. 675. H. Iwahara, T. Esaka, H. Uchida, and N. Maeda, Solid State Ionics, 3/4 (1981) 359. H. Iwahara, Solid State Ionics, 28-30 (1988) 573. N. Bonanos, B. Ellis, and M.N. Mahmood, Solid State Ionics, 28-30 (1988) 579. H. Uchida, N. Maeda, and H. Iwahara, Solid State lonics, 11 (1983) 117. T. Ohgi, T. Namikawa, and Y. Yamazaki, see Ref. 4.9, p. 357. T. Yajima, H. Iwahara, H. Uchida, and K. Koide, Solid State Ionics, 40/41 (1990) 914. T. Yajima and H. Iwahara, Solid State Ionics, 50 (1992) 281. T. Yajima and H. Iwahara, Solid State lonics, 53-56 (1992) 983. T. Scherban and A.S. Nowick, Solid State Ionics, 35 (1989) 189. H. Uchida, H. Yoshikawa, and H. Iwahara, Solid State Ionics, 35 (1989) 229. H. Uchida, H. Yoshikawa, T. Esaka, S. Ohtsu, and H. Iwahara, Solid State Ionics, 36 (1989) 89. T. Yajima, H. Kazeoka, T. Yogo, and H. Iwahara, Solid State Ionics, 47 (1991) 271. H.H. Huang, M. Ishigame, and S. Shin, Solid State Ionics, 47 (1991) 251. R.L. Cook, J.J. Osborne, J.H. White, R.C. MacDuff, and A.F. Sammells, J. Electrochem. Soc., 139 (1992) L19. M. Schwartz, B.F. Link, and A.F. Sammells, J. Electrochem. Soc., 140 (1993) L62. T. Scherdan, S.Q. Fu, and A.S. Nowick, see Ref. 4.231, p. 663.
Chapter 5 CATHODE 5.1 REQUIREMENTS The main function of the cathode is to provide reaction sites for the electrochemical reduction of the oxidant. Thus, the cathode material must be stable in the oxidant oxidizing environment and have sufficient electronic conductivity and catalytic activity for the oxidant gas reaction at the operating conditions. Since the SOFC operates at high temperatures (600 ~ to 1000~ the cathode must be chemically and thermally compatible with the other cell components, from room temperature to those operating temperatures and to the even higher temperatures at which the fuel cell is fabricated. The key requirements for the cathode in the SOFC are discussed below. This discussion is qualitative because the specific requirements depend on selected materials and cell and stack designs [5.1]. (i) Stability: The cathode must be chemically, morphologically, and dimensionally stable in the oxidant environment. The cathode material must have no disruptive phase transformation (involving large changes in molar volume) between room temperature and fabrication temperature. The cathode must maintain its desired microstructure in long-term operation; significant microstructural changes can cause degradation in cell performance. (ii) Conductivity: The cathode must possess sufficient electronic conductivity to support electron flow in the oxidizing environment at the operating temperature. In general, maximum possible cathode conductivity is desirable to minimize ohmic losses.
(iii) Compatibility: The cathode must be chemically compatible with other components, not only at the operating temperature, but also at the much higher temperature at which the fuel cell ceramic structure is fabricated. Chemical interaction or elemental interdiffusion between the cathode and adjoining components must be limited in order to minimize unacceptable occurrences such
Chapter 5
118
as second phase formation, stability reduction, change in thermal expansion, introduction of electronic conductivity in the electrolyte, etc. (iv) Thermal expansion: The thermal expansion of the cathode must match (from room temperature to operation and fabrication temperatures) that of other cell components to avoid cracking and delamination during fabrication and operation, including thermal cycling. (v) Porosity: The cathode must have sufficient porosity to allow gas transport to the reaction sites. The lower limit on porosity is set by mass transport considerations. (The porosity limit may be less critical for mixed conducting materials.) The upper limit is based on consideration of mechanical strength of the component. (vi) Catalytic activity: The cathode must have sufficient catalytic activity, thus low polarization, for the electrochemical reduction of the oxidant. In addition to these requirements, other desirable properties for the SOFC cathode are high strength and toughness, fabricability, and low cost. Because of the high operating temperature of the SOFC (600 ~ to 1000~ only noble metals and electronic or mixed conducting oxides can be used as cathode materials. Noble metals such as platinum and palladium are unsuitable for practical applications because of prohibitive cost. Many doped oxides are available, but only a few meet the requirements of thermal expansion match and compatibility with the electrolyte. At present, doped lanthanum manganite (LaMnO3) is most commonly used. 5.2 LANTHANUM MANGANITE Doped LaMnO3 has been extensively used as cathode material in the SOFC. This selection has been based primarily on three factors: high electrical conductivity in oxidizing atmospheres, adequate compatibility with Y 2 0 3 stabilized ZrO2 (YSZ) electrolyte, and acceptable thermal expansion match with other cell components. Other properties of LaMnO3 are tailored to meet the requirements for SOFC applications.
5.2.1 Preparation Various methods have been used for the fabrication of LaMnO3 cathodes (for references, see fabrication sections of Chapter 9). In the sealless tubular design, LaMnO3 cathode layers are deposited on the porous support by ' slurry
Cathode
119
coating. In the segmented-cell-in-series design (banded configuration), the cathode is made by flame spraying ceramic powders onto the surface of the electrolyte. In the monolithic design, the cathode layer is formed by tape calendering (with the other components) and then cofired at elevated temperatures. In the flat-plate design, the cathode is applied on the electrolyte by various techniques such as casting, printing, spraying, and depositing. Figure 5.1 shows an example of the microstructure of LaMnO3 cathode made by tape calendering. In general, the processing conditions of each fabrication method are tailored to produce the required cathode structure. Each method is also designed such that no conditions in any preparation step destroy desired characteristics of the LaMnO3 material. Recently, several new techniques have been investigated for the fabrication of the cathode, especially as thin films. For example, thin LaMnO3 layers have been formed on YSZ by electroless deposition from a solution containing manganese ions, lanthanum ions, and an oxidizing agent [5.2]. A pyrosol derived method has been applied to produce strontium-doped LaMnO3 films 5 to 10 ~m thick for SOFC cathode applications [5.3]. LaMnO3 layers have also been prepared by techniques such as oxidation plating [5.4], electrochemical deposition [5.5], vacuum evaporation [5.6], and film coating
[5.71. Many fabrication methods for LaMnO3 use fine powders as starting materials. LaMnO3 powders are commonly prepared by the amorphous citrate (Pechini or liquid mix) process [5.8]. The process involves dissolving appropriate proportions of salts of desired metal elements in a citric acid/ethylene
Figure 5.1. Microstructure of LaMnO~ cathode made by tape calendering
120
Chapter 5
glycol solution. The solvent is evaporated, and a transparent amorphous resin containing a homogeneous mixture of the metals is formed. The resin is then decomposed by heating to remove the organics and produce the desired oxide. The amorphous citrate or liquid mix process involves two basic chemical reactions: (i) complexation or chelation between metal ions and citric acid, and (ii) polyesterification of complexes with ethylene glycol. The complexation and polyesterification reactions preserve the homogeneity of the metal salt solution in a gel. As a result, powders produced have high surface area and precise compositional stoichiometry. Polymerization and decomposition conditions of the amorphous citrate process are often tailored or modified to achieve the desired characteristics of the oxide powder product [5.9-5.12]. The process has also been modified by changing the citric acid/ethylene glycol ratio of the preparation solution [5.9, 5.11, 5.13, 5.14]. In addition to the Pechini process, several other methods have been developed for the synthesis of LaMnO3 powders. The freeze drying method produces LaMnO3 with a very high surface area (14 to 32 m2/g) by spraying a suitable nitrate solution into a cryogenic medium [5.15]. The spray pyrolysis process prepares fine oxide powders by thermally decomposing aqueous nitrate solution droplets in a hot reaction chamber [5.16-5.19]. The sol-gel process produces strontium-doped LaMnO3 powder (particle size of 0.3 to 0.7/zm and surface area of 17.5 to 23.5 m2/g) using polyacrylic acid to make a gel [5.20]. The glycine/nitrate combustion method prepares extremely fine LaMnO3 materials by evaporating and autoigniting an aqueous metal nitrate/glycine solution [5.21].
5.2.2 General properties, phase transformation, and stoichiometry LaMnO3 belongs to the class of perovskite oxides of the general formula ABO 3. The cubic perovskite structure comprises three interpenetrating threedimensional networks" two consisting of the separate A and B cations and the third of corner-sharing 06 octahedra. Thus, the ideal structure of LaMnO3 can be described as a MnO6/2 framework of corner-shared octahedra that contains lanthanum cations within 12-coordinate sites (Figure 5.2). The cubic structure of LaMnO3 may undergo atomic distortion leading to orthorhombic or rhombohedral unit cells. LaMnO3 melts at about 1880~ [5.22]. The phase diagram of the La203-Mn203 system is shown in Figure 5.3 [5.22]. Table 5.1 lists the properties of LaMnO3.
121
Cathode
Q
La
Mn06
Figure 5.2. Meal perovskite structure of LaMnO 3
2600
"
P - perovskite-type LaMn03 phase 1 - liquid o - observed -- - estimated
La203", 2200 ,
liquid
v
,
- - ........
-''
,-
P+l
'. '11
tt. I
"'. p
liquid x x
",
4-
,
1800
xx x
liquid
',
P
+
- -" - f +
,~" M,,,_q,
c-Mn304
UJ
I--1400
La203
1000
0.0
/p~
P
o
o
_ _
+
.l
. . . . . .
t.
P + t Mn304
o L__i _~..1]~___~ ~ .
0.2
.
.
.
.
.
.
.
Mn~ 03~
.
0.4
0.6
0.8
1.0 Mn20s
La203 M n / ( L a + Mn)
Figure 5.3. Phase diagram of a Mn203-La203 system [5.22]
Chapter 5
122
TABLE 5.1
Properties of LaMnO3 Melting point, ~ Density, g/cm3 Thermal conductivity, W/cm.K Thermal expansion coefficient, 10 .6 cm/cm.K (25 o to 1100~C) Standard enthalpy of reaction, kJ/mol (from LazO3(s), MnO(~), and O2(g), 1064 to 1308 K) Standard entropy change, J/mol.K (from La203(~), MnO(s), and O2(g), 1064 to 1308 K) Strength at 25 ~ (30 % porosity), MPa
1880 6.57 0.04 11.2
[5.22]
[5.221 [est.]
-168
[5.24]
-65
[5.24]
25
[est.]
[5.231
Undoped stoichiometric LaMnO3 is orthorhombic at room temperature [5.25,5.26] and shows an orthorhombic/rhombohedral crystallographic transformation at about 600~ [5.26]. This transformation has been attributed to the oxidation of some Mn 3§ to Mn 4§ ions [5.26]. Thus, the orthorhombic/ rhombohedral transition temperature is dependent on the Mn 4§ content, and therefore, very sensitive to the stoichiometry of the material, especially that of oxygen. For example, various transformation temperatures (285~ [5.27], 300~ [5.28], 387~ [5.29], 450~ [5.25]) have been reported for LaMnO3 samples having different degrees of oxygen nonstoichiometry. At high Mn 4§ content or high oxygen-excess level (i.e., LaMnO3+~ with t5 > 0.1), the compound is rhombohedral at room temperature [5.30-5.32]. Doping such as substituting a lower-valence cation for lanthanum and manganese sites increases the Mn 4§ concentration in LaMnO3, thus affecting the transformation temperature. For example, strontium doping and calcium doping change the structure of LaMnO3 from orthorhombic to rhombohedral at room temperature [5.31,5.33,
5.341. LaMnO 3 can have oxygen excess, stoichiometry, or deficiency depending on the preparation conditions such as firing atmosphere, temperature, and time. For example, LaMnO3.~5 (30% Mn 4§ concentration) is obtained when heated at 1100~ in oxygen for 6 days [5.26]. On the other hand, LaMnO:.99 is obtained when quenched from 1300~ in air [5.31]. At high temperatures, the oxygen stoichiometry of LaMnO3 varies as a function of oxygen partial pressure and
Cathode
123
temperature. For example, at 1200~ the oxygen stoichiometry of LaMnO3 ranges from 3.079 to 2.947 under oxygen partial pressures of 1 to 10-116~ atm ( 1 0 5 tO 10 -6.6o Pa) [5.35]. In oxidizing atmospheres, LaMnO3 has oxygen excess and the amount of excess oxygen depends on temperature. In reducing atmospheres, the material becomes oxygen deficient. Under highly reducing conditions, LaMnO3 dissociates into La203 and MnO; however, the dissociation is reversible [5.36]. For doped LaMnO3, the level of oxygen excess-decreases with increasing dopant content [5.36,5.37]. Thus, LaMnO3 containing 20 mol % calcium dopant has no oxygen excess even at high oxygen activities [5.38]. Figures 5.4, 5.5, and 5.6 show how the oxygen content of undoped and strontium-doped LaMnO3 varies as a function of oxygen partial pressure, temperature, and dopant concentration [5.36]. For SOFC applications, significant changes in oxygen stoichiometry of LaMnO3 (especially during fabrication) must be avoided to minimize undesired dimensional changes [5.39]. In addition to oxygen nonstoichiometry, LaMnO3 can also exhibit lanthanum deficiency or excess. LaMnO3 with lanthanum excess may contain La203 second phase, which tends to be hydrated to La(OH)3. This hydration is undesirable for SOFC applications because it can cause disintegration of the sintered LaMnO3 structure. LaMnO3 can have up to about 10% lanthanum deficiency without second phase formation [5.31]. Above this level, Mn304 is present as the second phase. In general, it is very difficult to prepare stoichiometric LaMnO3; the undoped material synthesized under normal conditions often possesses about 0.2 mol % lanthanum vacancies [5.36]. 3.10 3.08 3.06
zx 1000oc 91100~ a 1200~
Z
I.-tUZO3'04 1 0 3.02 3.00 >" I 0 2.98 i "
=,.. =.p
, ./-,,=
y y / . . ~ .
r'l
X
/2
'l'
l
-16 -14 -12 -110 ]8 -6 -4 ]2 0 LOG OXYGEN PARTIAL PRESSURE, atm (1.01 X 105 Pa)
-18
Figure 5.4. Oxygen content of undoped LaMnO~ as a function of oxygen partial pressure and temperature [5.36]
124
Chapter 5
3.10
"6 E k-, 3.00 Z Ill FZ 0 0 Z tu 2.90 (9 >• 0
.
.
.
.
.
.
.
.
.
.
_j;
.
.=.=~A-.,=- ~ , ~ = = f
f
~.=r
/
/
.- o
o-
/=
oo
a IO00oc
/ /~a ~
91 1 0 0 ~
.
o
1200~
D
2.80 . -18
-16
-114
I
I
-12
-10
"1
I
-8
-6
-4
:2
0
LOG OXYGEN PARTIAL PRESSURE, atm (1.01 X 106 Pa)
Figure 5.5. Oxygen content of Lao9SroiMnO3 as a function of oxygen partial pressure and temperature [5.36]
3.10 ,
~. 3 . 0 0 Z
~=~
Z 0 2.900 Z ILl (9 >-
L
X0
| i , IiIll~-II~I''~ - -
_,+A-_
,+, 9 ,v@
A LaMn0a 9 Lao.agSro.olMnOa o Lao.e6Sro.o~MnOa
2.80-
9 Lao.ooSro.+oMnOa 9
2.70 . !8
j
-;6
o Lao eoSro.2oMn0a
-1'4
-1'2
-;o
;8 .... -'6
-~,
-~
LOG OXYGEN PARTIAL PRESSURE, atm (1.01 x 106 Pa)
Figure 5.6. Oxygen content of Lal.xSrxMnOs as a function of oxygen partial pressure at 1000~ [5.36]
125
Cathode
The defect chemistry of undoped and doped LaMnO3 has been studied [5.29, 5.36, 5.38, 5.40-5.46]. A defect model based on unassociated and randomly distributed point defects (metal and oxygen vacancies) has been proposed. In this conventional defect structure model, the formation of metal vacancies in the high oxygen activity region (the oxide has oxygen excess) can be expressed by the following equation (using Kr6ger-Vink notation):
+ +/ CMn / // 6MnMn +2230= CGa
6Mndn + 30 o
(Eq. 5.1)
Assuming equal concentration of vacant lanthanum and manganese sites, the concentration of metal vacancies is thus proportional to the 3/4 root of the oxygen partial pressure (Region I). As the oxygen activity decreases, the oxide becomes stoichiometric (Region II). At low oxygen activities, the oxide is oxygen deficient, and oxygen vacancies are the predominant point defects. The formation of oxygen vacancies can be written as 10 2 2Mnr~n + Oo = 2Mnr~n + Vo + ~-
(Eq. 5.2)
Under these conditions, the concentration of oxygen vacancies is inversely proportional to the 1/2 root of oxygen partial pressure (Region III). At sufficiently low oxygen activities, the concentration of oxygen vacancies is constant; thus, the oxygen nonstoichiometry is independent of the oxygen partial pressure. Under these conditions, the concentration of electron holes is proportional to the 1/4 root of oxygen partial pressure (Region IV). Figure 5.7 summarizes the variation of the oxygen stoichiometry of LaMnO3 as a function of oxygen partial pressure according to the proposed model.
Figure 5. 7. Oxygen content as a function of oxygen activity as predicted from defect model
Chapter 5
126
In general, LaMnO3 exhibits a defect chemistry very close to that shown in Figure 5.7 for high oxygen activity regions (Region I, II, and III) (see Figures 5.4, 5.5 and 5.6). Other experimental results support the basis of the model: lanthanum and manganese vacancies are randomly distributed in equal amounts in oxygen-excess LaMnO3 [5.47,5.48]. However, the material behavior deviates significantly from the model predictions for low oxygen activity regions. (No region IV is observed.) This deviation has been explained by a change in the manganese valency such as the thermally excited disproportionation of Mn 3§ into Mn 2§ and Mn 4§ ions [5.36,5.41-5.43,5.48]. Other models based on defect clusters have been suggested to explain the behavior of oxygen-deficient LaMnO3 in the low oxygen activity regimes [5.41,5.45]. For example, association of oxygen vacancies and dopant ions has been proposed [5.45].
5.2.3 Stability At the SOFC operating temperature, LaMnO3 is stable in oxidizing atmospheres but decomposes under highly reducing conditions. The lowest oxygen partial pressure before LaMnO3 dissociates into multiple phases is termed the critical oxygen partial pressure. At 1000~ the critical oxygen partial pressure for undoped LaMnO3 is about 10-14 to 10-~5 atm (10 .9 to 10-1~ Pa) [5.24,5.49-5.52]. The critical oxygen partial pressure for LaMnO3 depends on temperature, shifting to higher values at higher temperatures. At the same temperature, this critical pressure increases with increasing dopant concentration [5.36]. Thus, a high dopant content generally results in reduced stability for the LaMnO3 compound. Figure 5.8 shows, as an example, the critical oxygen partial pressure of La~_xSrxMnO3_~ as a function of temperature and dopant content [5.40]. At the SOFC operating temperature, LaMnO3 decomposes directly to La203 and MnO at the critical oxygen partial pressure [5.35,5.49,5.53]. However, at lower temperatures (350 ~ to 600~ the material tends to transform to other phases such as LazMnO4, La8Mn8023, LanMn4Oll [5.54,5.55]. Nonstoichiometry can influence the stability of LaMnO3. Lanthanum excess tends to precipitate as La203, causing hydroxide formation and subsequent disintegration of sintered LaMnO3 structures at room temperature [5.56]. Lanthanum-deficient LaMnO3 is more stable; however, the lanthanum deficiency must be less than 10% to prevent Mn304 formation [5.31]. LaMnO3 with lanthanum deficiency is recommended for use in SOFCs.
Cathode
127
T, ~ 1200
1000
i
T
o
-t-
600
,
: Lao.6Sro.4Mn03.6
- 0 - : Lao.eSro.2Mn03_ 6
X
0
BOO
-0-
-5
: Lao.oMn03.6
zx :, LaMn03_6
v
E IO
u~ fie ::=) (/) u) Ill
-10
-15
iv,
o. _1
_~ I-<
-2o
O.
z
-25
(9 >. X 0 (9 0
-30
Ill
...I
=
i
i
i
|
l
6
7
8
9
10
11
|
12
13
I/T, 10 .4 K -I
Figure 5.8. Criticaloxygen partial pressure of LavxSr~l/ln03 [5.40]
5.2.4 Electrical conductivity LaMnO3 has intrinsic p-type conductivity due to the formation of cation vacancies. The material has an electrical conductivity of about 10 -4 f]-lcm-l at room temperature and about 0.1 ~2-1cm-1 at 700~ The electrical conductivity of LaMnO3 has been enhanced for SOFC applications by substituting a lowervalence cation on either the A or B sites. LaMnO3 has been substituted with various cations such as barium [5.575.59], calcium [5.16,5.42,5.57,5.60-5.64], chromium [5.65-5.67], cobalt [5.25,5.68-5.72], copper [5.73], lead [5.74], magnesium [5.75], nickel [5.28,5.30], potassium [5.76,5.77], rubidium [5.77], sodium [5.77,5.78], strontium [5.29,5.31,5.34,5.78-5.87], titanium [5.58], and yttrium [5.88]. Besides electrical conductivity, many of these substituents are used to modify other properties (e.g., thermal expansion) of LaMnO3. Presently, strontium and calcium dopants are most commonly used in SOFCs because LaMnO3 doped with these cations has high electronic conductivity in oxidizing atmospheres and relatively matches the thermal expansion of other cell components.
128
Chapter 5
Strontium doping enhances the electronic conductivity of LaMnO3 by increasing the Mn 4+ content by the substitution of La 3§ by Sr 2+" xSrO
x_3+
~
2+-= ,r
3+ ,= .
4+,--,
LaMnO 3 __, La~_x~rx~vm~_xMnx u 3
(Eq. 5.3)
The electronic conductivity of strontium-doped LaMnO3 takes place via the small polaron conduction mechanism. Figure 5.9 shows the temperature dependence of the conductivity of both undoped and strontium-doped LaMnO3 [5.29]. For undoped LaMnO3, the break in the conductivity plot seen in Figure 5.9 can be explained by the orthorhombic/rhombohedral crystallographic transition. At temperatures below 1000 ~ plots of In aT (where tr is the conductivity and T is the temperature) vs 1/T are linear, as predicted by the following equation derived for the small polaron conduction: (Eq. 5.4)
tr = (AJT)exp(-E/KT)
where A~ is the preexponential factor, K the Boltzmann constant, and E~ the activation energy for conduction. The Eo values calculated from the slopes of the plots are 18.3, 18.3, 15.4, and 8.7 kJ/mol for undoped, 5, 10, and 20-mol%strontium-doped LaMnO3. For LaMnO3 doped with < 20 mol% strontium dopant, the conductivity of the material increases with increasing temperature and increasing strontium concentration at temperatures below 1000~ The conductivity becomes nearly constant at temperatures above 1000 oc, suggesting a semiconducting-to-metallic transition [5.29,5.31]. The material may show the metallic conduction behavior at a lower transition temperature depending on the 14
~1~11~ II - III.. ii1..._ B...... _ "7,
Ell
'7,
C o LaMn03 ~ 0
_d
8
A Lao.96Sro.o~Mn03 0
"o. ~"
Lao.9oSro.loMnO 3
I
-.
" Lao.eoSro.2oMn03
"-. "0
9
12
15
lIT,
18
21
24
1 0 .4 K ~
Figure 5.9. Electrical conductivity of undoped and strontium-doped LaMnO~ [5.29]
Cathode
129
lanthanum stoichiometry [5.82]. As the strontium content is > 20 to 30 mol %, the metallic-type conduction is then observed for LaMnO3 over the entire temperature range [5.31,5.84,5.86]. The variation of the electrical conductivity of La~_xSrxMnO3 with strontium content appears to exhibit a maximum. At the SOFC operating temperatures (600 ~ to 1000~ the strontium level where the maximum conductivity is observed is about 55 mol % [5.86]. Similar to strontium doping, calcium doping significantly enhances the electronic conductivity of LaMnO3, and the conduction of the calcium-doped compound also occurs via a small polaron hopping mechanism. At a calcium content of < 50 mol%, the conductivity of La~_xCaxMnO3 increases with increasing temperature and shows a metallic-type conduction transition at about 600~ to 700~ [5.16, 5.89]. Above 60 mol % calcium, the conduction behavior of the material is entirely metallic (negative temperature dependence) [5.89]. At the SOFC operating temperature, the maximum conductivity of La~_xCaxMnO3 occurs at 50 mol % calcium [5.89]. Table 5.2 lists conductivity data for several doped LaMnO3 compounds. It should be noted that the values given in Table 5.2 are very much dependent on preparation conditions and material stoichiometries; other values have been reported in the literature. TABLE 5.2
Conductivity Data for Doped LaMnO3 Dopant (MO)
SrO SrO SrO CaO CaO NiO SrO,Cr203
SrO,Co203
Composition Conductivity,1000~C (mol % MO) (fl-lcml)
10 20 50 25 45 20 10,20 20,20
130 175 290 165 240 100 25 150
Activationenergy (kJ/mol)
Ref.
15.4 8.7 4.5 11.6 7.9 18.6 13.5 -
[5.291 [5.291 I5 151
[5.75J [5.751
[5.281 [5.6o]
[5.7Ol
130
Chapter 5
The electrical conductivity of undoped and doped LaMnO3 decreases significantly in the low oxygen partial pressure region. The dependence of electrical conductivity of LaMnO3 on oxygen partial pressure has been correlated to the material defect structure [5.29,5.38]. For example, the defect reaction for La~_xSrxMnO3_~ may be represented by 2MnMn + O~ = 2MnMn + V~ + 71o 2
(Eq. 5.5)
The equilibrium constant in terms of mole fraction is given as (1 -x+2~)2(~)Po/~
K =
(Eq. 5.6)
(x-2tS)2(3 -~i)
This equation can be approximated as (Eq. 5.7)
g
(x-2tS) 2
The electrical conductivity a of the material is given by (Eq. 5.8)
tr = e ~ p
where e is the electron charge, /z the mobility, and p the carrier concentration (p = x - 26). By solving Eq. 5.7 and combining it with Eq. 5.8, the conductivity becomes I"1' D 1/2 [ [ ~
~. r , , " D - 1 / 2
a = e 4 K , o, twx~xro,
+ 1)1/2 - 1]
(Eq. 5.9)
In the high oxygen activity region, x approaches zero; Eq. 5.9 then reduces to Eq. 5.8. Thus, the conductivity is independent of oxygen partial pressure. However, in the low oxygen activity region, Eq. 5.9 becomes _
,,
X
= eg~-~-g)
\1/2r~1/4
ro~
(Eq. 5.10)
The computed conductivity for strontium-doped LaMnO3 as a function of oxygen activity shows excellent agreement with the experimental data (Figure 5.10).
131
Cathode
2.4 2.2 o
2.0 1.8 IL)
~~~
z~ 1.6 z
/
1.0 // .
,1000~ = 1100~ * 1200~
P/
0 (9 1.4 (9 0 1.2 6
/
-14
-;2
-10
. -6
-'8
. -4
:2
0
LOG OXYGEN PARTIAL PRESSURE, atm (1.01 x 106 Pa)
Figure 5.10. Conductivity as a function of oxygen partial pressure for LaosSro~/lnO3 at various temperatures [5.29]
Similar results are also obtained for undoped LaMnO3 (Figure 5.11). As seen from Figures 5.10 and 5.11, the electrical conductivity of both undoped and strontium-doped LaMnO3 shows little dependence on oxygen partial pressure in the range of high oxygen activity, and this range narrows with increasing temperature. As the oxygen activity decreases, the conductivity decreases according to Eq. 5.10 and then drops abruptly (due to dissociation of LaMnO3 phase) at highly reducing conditions (critical oxygen partial pressures).
2.0
u O
~
1.9
\
-
.
m
> o z
1.8 ~//~== / ~
O o 1.7 (9 o
a 1000~ = 1100~ o 1200oc
1.6 -16 -14 -12 -10 -8 -6 -4 -2 0 LOG OXYGEN PARTIAL PRESSURE, atm (1.01 x 105 Pa)
Figure 5.11. Conductivity as a function of oxygen partial pressure for undoped LaMnO 3 at various temperatures [5.29]
132
Chapter 5 5.2.5 Chemical interaction
The high fabrication and operation temperatures of the SOFC raise concerns regarding the chemical compatibility of LaMnO3 cathode with other cell components, especially the YSZ electrolyte. Manganese is known to be a mobile species at high temperatures and can easily diffuse into the electrolyte, changing the electrical characteristics or the structure of both the cathode and the electrolyte [5.90]. Fabrication temperature is generally limited to below 1400~ to minimize this migration. At temperatures below 1000~ manganese migration is negligible [5.91,5.92], and there is no report on any significant manganese effects for SOFCs operated up to 10,000 h. The chemical interaction between LaMnO3 and YSZ has been studied at SOFC operating and fabrication temperatures. No significant reactions between LaMnO3 and ZrO2 have been observed at temperatures below 1100 ~ to 1200~ above 1200~ the manganite reacts with ZrO2 to produce La2Zr207 [5.93-5.97]. Other reaction products (e.g., SrZrO3 and other zirconate phases) may also form with LaMnO3 containing high dopant content [5.94, 5.97-5.101]. The interaction is significant at high temperatures and long times. For example, a layer of La2Zr207 up to 5 /~m thick can form at the LaMnO3/YSZ interface if fired at 1450~ for 48 h [5.97]. The formation of La2Zr207 and other phases at the LaMnO3 cathode/YSZ electrolyte interface is undesirable in SOFCs: these compounds can deleteriously affect the performance of the cell because they can both act as an insulating layer and create thermal stresses at the interface. The electrical conductivity of La2Zr207 and SrZrO3 is several orders of magnitude lower than that of YSZ and the thermal expansion coefficients of the materials are significantly lower than that of YSZ [5.102-5.106]. The LaMnO3/YSZ interaction appears to proceed via the unidirectional diffusion of manganese, lanthanum, or dopant cation (e.g., strontium, calcium) into the YSZ [5.107,5.108]. A proposed mechanism for the interaction suggests high manganese diffusion into YSZ, resulting in lanthanum excess at the interface, which then reacts with the YSZ to form zirconates [5.108]. The presence of a dopant in LaMnO3 suppresses the manganese migration; thus, substitution of lanthanum in the manganite with a low dopant concentration reduces the La2Zr207 formation [5.93,5.108]. A high dopant content results in the formation of other phases such as SrZrO3, CaZrO3. Figure 5.12 shows, as an example, how the dopant content influences the reactivity of LaMnO3 and the reaction products formed at different temperatures [5.101]. The interaction
133
Cathode
1700
La2ZraO~ / E ,.d nr :::) I-,a:
1500
LaaZr20~
SrZr03
nr I.,U n
~ 1300
1100 0.0
. 0.1
.
. 0.2
.
. 0.3
. 0.4
0.5
0.6
0.7
S T R O N T I U M C O N T E N T , mol
Figure 5.12. Diagram showing reaction products formed from La~_xSr~/InO3 and YSZ at different temperatures [5.101]
between LaMnO3 and YSZ is also influenced by the stoichiometry of the perovskite material. Lanthanum deficiency reduces the reactivity of LaMnO3 toward YSZ [5.93,5.94,5.109]. The interaction between LaMnO3 and YSZ has been examined by thermodynamic analysis of various equilibria in terms of chemical potentials of all elements involved [5.110-5.119]. Figure 5.13 is an example of a constructed triangle diagram based on such analysis. The diagram predicts the various processes taking place between strontium,calcium-doped LaMnO3 and YSZ at 1400~ in air. Chemical potential diagrams are also constructed. The chemical potential diagram of the La-Mn-Zr-O system at 1300 ~ is shown in Figure 5.14. This diagram also takes into account the dissolution of lanthanum and manganese into YSZ and the lanthanum nonstoichiometry in LayMnO3_~ (since manganese is known to diffuse into the YSZ, and the lanthanum deficiency in LaMnO3 affects its reaction with YSZ). The diagram suggests that the LazZrzO7 formation takes place for y > 0.86, whereas the manganese dissolution may become significant for y < 0.86. The LazZrzO7 formation gives rise to the lanthanum depletion in the LaMnO3 phase, resulting in a decrease in lanthanum stoichiometry y. The manganese dissolution gives rise to the manganese depletion in the perovskite. When LaMnO3 is doped with a lower-valence cation such as strontium, zirconates formed change with strontium content (from La2Zr207 to SrZrO3) (Figure 5.15). La~_xSrxMnO3 can be in equilibrium with La2Zr207 or SrZrO3 or both, depending on the particular composition.
134
Chapter 5
LoMnO 3
y
~
~_~(Sr,C o)ZrOq
CoMnO 3
SrMnO 3
Figure 5.13. Diagram showing possible reactions between strontium, calcium-doped LaMnO 3 and YSZ at 1400 ~C [5.115]
10
r~ '
(.9 0
--
6
4
o
2
00J---~--
+ -'-
I ~ ~ ~ - ~ - ~ I _ ~
"--
i
-~-
l-Jj
I
i
.... I
I
o ~./41o d~ c~do .., , "
II
Mn3u4 H .
-2
10
12
14 LOG
16
18
20
22
aMn/azr
Figure 5.14. Chemical potential diagram of a La-Mn-Zr-O system at 1300~ [5.117] (a is the activity)
Cathode
135
15 . . Z -J~.---
I
i lO
9
_J
SrO
I AIB
I
.. ^ ~ 1
p"o12"" % ,
/
/
/
/
/ /
: I i
I
.'~,"
,,.[-SrZrO 3 I .b ,, [ formotion!_//, , / .O'b" stockingl - -." ," .,~/~e~
~t
~I..'.'" J A .~'
V)
(.9 O _.J
..........
5 ;
"i
i ~_ JA-_Si!e ii '"
[L~ /f~176
Lo203 5
i
~
(Lo,S")Mn%i 10 LOG
15
" M n30/. ,
20
aMn/aLa
Figure 5.15. Chemical potential diagram of a La-Sr-Mn-Zr-O system at 1300~ [5.118]
In addition to reaction with YSZ, LaMnO3 may react with doped LaCrO3 when in contact with this interconnect material at high temperatures. Strontium and calcium dopants in LaCrO3 tend to migrate to the interface to form compounds such as (Sr,La)3Mn207 and (Ca,La)3Mn/O7 [5.117,5.120]. The interaction may also form solid solutions between LaMnO3 and LaCrO3 at the interface [5.121]. 5.2.6 Thermal expansion The thermal expansion coefficient of undoped LaMnO3 (La0.99MnO3) from 25~ to 1100~ is 11.2• x 10 -6 cm/cm.K [5.23]. Lanthanum deficiency and oxygen nonstoichiometry appear to lower the thermal expansion of the material [5.31,5.122]. Strontium doping increases the thermal expansion coefficient of LaMnO3, and the coefficient increases with increasing strontium dopant content [5.23]. Substitution for lanthanum with smaller cations, such as calcium or yttrium, lowers the thermal expansion coefficient of LaMnO3 [5.16,5.88,5.89]. For
Chapter 5
136
example, the average thermal expansion coefficient of Lao.9Cao.lMnO 3 from room temperature to 1000~ is about 10.1 x 10 -6 cm/cm-K [5.16]. The coefficient of calcium-doped LaMnO3 is higher at higher calcium concentration [5.16, 5.122] (10.1 to 11.4 x 1 0 -6 cm/cm.K for calcium content ranging from 10 to 50 mol% [5.16]). Forming solid solutions of LaMnO 3 with LaCoO3 and LaCrO3 leads to higher thermal expansion coefficients [5.67,5.69,5. 70,5.123]. Figure 5.16 shows the variation of the thermal expansion of Lao.5Sro.sMnO3-LaCoO3 solid solutions as a function of cobalt content [5.70]. Tables 5.3 and 5.4 list selected thermal expansion data for doped LaMnO3. 26 Z
uJ o U..
9Powder (X-Ray diffractometry)
LL
l
22
UJ 0
t
uu z
/
II
t
=
E
o
o4 z ~o x'-
18
i
t I
W _J
EJ
14
ii
"
"
II -1-
I
10 0,0
0.2
0,4
0,6
0.8
1.0
COBALT CONTENT, mol
Figure 5.16. Thermal expansion coefficients of Lao.sSro.sMnl.xCoxO3 compounds [5.70] TABLE 5.3 Thermal Expansion Coefficient of Lal_xSrxMnO3 (25 ~ to ll00~ [5.23]
Composition
Thermal expansion coefficient
(10.6 cm/cm.K)
Lao.99MnO3 Lao.94Sro.osMnO3 Lao.s9Sro.loMnO3 Lao.79Sro.2oMnO3 Lao.69Sro.3oMnO3
11.2 11.7 12.0 12.4 12.8
Cathode
137
TABLE 5.4
Thermal Expansion Coefficients of Doped LaMnO3 Composition
Lao.9Sro.lMnO3 Lao.sSro.sMnO3 Lao.9Cao.lMnO3 Lao 5Cao.sMnO3 Lao.nYo.1Sr0.sMnO3 Lao.vSro.3Mno.7Cro.303 Lao.8Sro.2Mno.7Coo.303
Thermal expansion coefficient (10.6 cm/cm.K)
Ref.
12.0 13.2 10.1 11.4 10.5 14.5 15.0
[5.23] [5.75] [5.16] [5.16] [5.88] [5.67] [5.70]
5.2.7 Other properties LaMnO3 can be sintered to full density at temperatures above 1250~ in air. Because the material can be easily densified under normal firing conditions, starting powders and processing procedures are often tailored to reduce the sinterability of LaMnO3 to produce a porous cathode structure (with required stability) for SOFC applications [5.17,5.124-5.126]. The sinterability of LaMnO3 depends on, among other factors, the dopant, dopant level, and cation nonstoichiometry of the material. For example, calcium-doped LaMnO3 is more sinterable than strontium- and barium-doped compounds [5.127]; LaMnO3 with a higher strontium dopant content requires a higher sintering temperature [5.81, 5.85,5.127]; and lanthanum deficiency improves the sinterability of LaMnO3
[5.81,5.127]. The oxygen diffusion in doped LaMnO3 plays an important role in the oxygen electrode reaction in SOFCs. The chemical diffusion coefficient of oxygen in Lao.79Sro.2oMnO3_~ and Lao 5oSro.5oMnO3_~ has been measured to be about 10.8 to 10 -6 cmZ/s in the temperature range of 700 ~ to 860~ indicating rapid oxygen transport [5.128, 5.129]. On the other hand, the oxygen self-diffusion coefficient has been found to be only about 10-~5 to 10~2 cm2/s for Lal_xSrxMnO3_~ at 700 ~ to 900~ [5.130-5.132]. This suggests that for SOFC applications, the LaMnO3 cathode porosity needs to be optimized to improve oxygen ion transport.
Chapter 5
138
Oxygen permeation in LaMnO3 has been described in terms of a point defect model [5.133]. 5.3 LANTHANUM COBALTITE Doped lanthanum cobaltite (LaCoO3) is another perovskite of interest as SOFC cathode material. The material belongs to the same class of oxide compounds as LaMnO3. LaCoO3 is rhombohedral from room temperature to 1000 oc [5.134-5.136]. The material rhombohedral structure may transform to a cubic phase; the transformation temperature depends on dopant content [5.135,5.136]. LaCoO3 has no oxygen excess but shows a large oxygen deficiency at high temperatures, especially when doped with a lower-valence cation such as strontium. At 1000~ the oxygen stoichiometry of undoped LaCoO3_6 ranges from 2.975 to 2.750 under oxygen partial pressures of 10.2 to 10.4 atm (103 to 10 Pa) [5.13 7]. At 800 ~C, the undoped compound is essentially stoichiometric. When doped with strontium, LaCoO3 becomes oxygen-deficient: the oxygen stoichiometry of La0.7Sr0.3CoO3_~ varies from 2.970 to 2.840 under oxygen partial pressures of 1 to 10.5 atm (105 to 1 Pa) [5.137]. The oxygen deficiency of the cobaltite increases with increasing temperature, increasing dopant content, and decreasing oxygen partial pressure [5.136-5.142]. The oxygen nonstoichiometry in LaCoO3 is inversely proportional to the l/ruth power of oxygen partial pressure. The values of 1/m have been found to be about 0.45 for undoped LaCoO 3 [5.143] and about 0.13 for Lao.7Sr0.3CoO 3 [5.140]. (i) Stability: LaCoO3 is stable in oxidizing atmospheres but decomposes in reducing environments. The material is less resistant toward reduction, when compared with LaMnO3. At 1000~ LaCoO 3 dissociates into other phases at the critical oxygen partial pressure of less than 10 -7 atm (10 .2 Pa) [5.49,5.52,
5.144, 5.145]. (For comparison, LaMnO3 decomposes at oxygen partial pressure of 10-~5 atm or 10-~~Pa.) Doping reduces the stability of LaCoO3, and the critical oxygen partial pressure shifts to higher values with increasing dopant content
[5.146]. (ii) Conductivity:
LaCoO 3 has been shown to have intrinsic p-type conductivity, and the electrical conductivity can be enhanced by substituting a lower-valence ion on the lanthanum site. Strontium and calcium are the most commonly used dopants for LaCoO 3. The conductivity of Lao.8Sr0.2CoO3_~ and Lao.8Cao.2CoO3_~ at 1000~ is 1200 f~-~cm-~ [5.70,5.135,5.136] and 800 fl-~cm-~ [5.147, 5.148], respectively. The conductivity of doped LaCoO3 increases with
Cathode
139
increasing dopant level and exhibits a maximum at 40 mol% for strontium [.5.136] and 30 mol % for calcium [5.138]. Undoped LaCoO3 shows a semiconducting-metallic conduction transition at about 800~ in an oxygen atmosphere [5.135]. Strontium and calcium doping appears to lower this transition temperature. Above 30 mol % strontium, the conductivity of the doped material is mainly metallic from room temperature to 1000~ [5.135,5.136,5.147]. (iii) Chemical interaction: LaCoO 3 interacts readily with YSZ to form La2Zr207 at high temperatures ( > 1100 oc) [5.116, 5.117]. Dopant present in LaCoO 3 may also react to produce other phases (e.g., SrZrO3 for strontium dopant [5.98, 5.102, 5.105]). Reaction products tend to form a multilayer reaction zone [5.116,5.149]. (iv) Thermal expansion: The average thermal expansion coefficient of L a C o O 3 is about 22 to 24 x 10 -6 cm/cm.K[5.147,5.149]. The coefficient can be modified by strontium [5.147], calcium [5.138,5.147], manganese [5.70], and nickel [5.149] substitution for lanthanum and cobalt. For example, the thermal expansion coefficient for LaCo0.6Nio.403 is about 17 x 10 -6 cm/cm.K[5.149]. In general, the thermal expansion coefficient of LaCoO 3 (even with doping) is significantly higher than that of YSZ electrolyte. 5.4 OTHER MATERIALS
A number of doped oxides have been proposed and investigated as SOFC cathode materials [5.150,5.151]. The disadvantages of most of these materials are thermal expansion mismatch, incompatibility with YSZ, and lack of conductivity. Early SOFCs used tin-doped indium oxide (In203) as the cathode material [5.152-5.1.54]. This material exhibits excellent electrical conductivity under fuel cell operating conditions and can be applied as thin film by the chemical vapor deposition method [5.155]. The material performed satisfactorily for up to 5000 h without degradation. However, In203 represents the most costly and least thermodynamically stable component in the SOFC. Therefore, In203 has been replaced by doped LaMnO3. Other materials containing In203, such as In203-PrO2-HfO 2, In203-PrO2-ZrO2, In203-ZrO 2 have also been proposed [5.1565.159]. Doped YMnO3, CaMnO3, and YFeO 3 compositions have been considered for possible SOFC cathode application [5.38,5.42,5.160-5.162]. Recently, compounds based on LaFeO3-LaCoO3 solid solutions have been studied as cathode materials in reduced-temperature SOFCs [5.163-5.165] due to their desirable mixed conducting properties [5.166,5.167]. Strontium-doped PrMnO3
140
Chapter 5
compositions show promise as a suitable cathode material for reduced-temperature applications [5.168].
RuO2/YSZ materials have also been evaluated for
SOFC cathode uses [5.169].
References 5.1
5.2 5.3 5.4 5.5 5.6
5.7 5.8 5.9
5.10 5.11 5.12 5.13 5.14 5.15 5.16
5.17
5.18 5.19
N.Q. Minh, in Science and Technology of Zirconia V, S.P.S. Badwal, M.J. Bannister, and R.H.J. Hannink (eds.), Technomic Publishing Company, Lancaster, PA, 1993, p. 652. T. Sasaki, Y. Matsumoto, J. Hombo, and M. Nagata, J. Solid State Chem., 105 (1993) 255. B. Gharbage, M. Henault, T. Pagnier, and A. Hammou, Mater. Res. Bull., 26 (1991) 1001. M. Nagata and H. Iwahara, Mater. Res. Bull., 28 (1993) 255. Y. Matsumoto, T. Sasaki, and J. Hombo, J. Electrochem. Soc., 138 (1991) 1259. H. Michibata, H. Tenmei, T. Namikawa, and Y. Yamazaki, in Proceedings of the First International Symposium on SolM Oxide Fuel Cells, October 16-18, 1989, Hollywood, FL, S.C. Singhal (ed.), Electrochemical Society, Pennington, NJ, 1989, p. 188. L.G.J de Haart, R.A. Kuipers, K.J. de Vries, and A.J. Burggraaf, see Ref. 5.6, p. 197. M.P. Pechini, U.S. Patent No. 3330697, July 11, 1967. H.U. Anderson, C.C. Chen, J.C. Wang, and M.J. Pennell, in Ceramic Powder Science III, G.L. Messing, S.I. Hirano, and H. Hausner (eds), American Ceramic Society, Westerville, OH, 1990, p. 749. M.S.G. Baythoun and F.R. Sale, J. Mater. Sci., 17 (1982)2757. L.W. Tai and P.A. Lessing, J. Mater. Res., 7 (1992) 502. N.M. Sammes and M.B. Phillipps, J. Mater. Sci. Lett., 12 (1993) 829. C. Marcilly, P. Courty, and B. Delmon, J. Am. Ceram. Soc., 53 (1970) 56. P. Sujatha Devi, J. Mater. Chem., 3 (1993) 373. D.W. Johnson, Jr., P.K. Gallagher, F. Schrey, and W.W. Rhodes, Am. Ceram. Soc. Bull., 55 (1976) 520. M. Fandel, J. H6schele, W. Sch/ifer, and R. Schmidberger, in Euro-ceramics Vol. 2, Properties of Ceramics, G. de With, R.A. Lerpstra, and R. Metselaar (eds.), Elsevier Applied Science, London, U.K., 1989, p. 2.236. M.R.F. Kuntz, in Proceedings of the Third International Symposium on Solid Oxide Fuel Cells, May 16-21, 1993, Honolulu, HI, S.C. Singhal and H. Iwahara (eds.), Electrochemical Society, Pennington, NJ, 1993, p. 301. I.A. Aksay, G.D. Maupin, C.B. Martin, R.P. Kurosky, and G.C. Stangle, U.S. Patent No. 5061682, October 29, 1991. N. Christiansen and P. Gordes, in Proceedings of the Second International Symposium on Solid Oxide Fuel Cells, July 2-5, 1991, Athens, Greece, F. Grosz,
Cathode
5.20 5.21 5.22
5.23 5.24 5.25 5.26 5.27 5.28
5.29 5.30 5.31 5.32 5.33 5.34 5.35 5.36
5.37
5.38 5.39
5.40 5.41
141
P. Zegers, S.C. Singhal, and O. Yamamoto (eds.), Commission of the European Communities, Luxembourg, 1991, p.495. H. Taguchi, D. Matsuda, and M. Nagao, J. Am. Ceram. Soc., 75 (1992) 201. L.A. Chick, L.R. Pederson, G.D. Maupin, J.L. Bates, L.E. Thomas, and G.J. Exarhos, Mater. Lett., 10 (1990) 6. J. van Roosmalen, Some Thermochemical Properties of (La, Sr)Mn03+ ~as a Cathode Material for Solid Oxide Fuel Cells, Netherlands Energy Research Foundation ECN, Petten, The Netherlands, 1993. S. Srilomsak, D.P. Schilling, and H.U. Anderson, see Ref. 5.6, p. 129. O.M. Sreedharan, P. Pankajavalli, and J.B. Gnanamoorthy, High Temp. Sci., 16 (1983) 251. G.H. Jonker, J. Appl. Phys., 37 (1966) 1424. B.C. Tofield and W.R. Scott, J. Solid State Chem., 10 (1974) 183. G.V. Subba Rao, B.M. Wanklyn, and C.N.R. Rao, J. Phys. Chem. Solids, 32 (1971) 345. I.Ya. Lyubkina and I.F. Kononyuk, Inorg. Mater. (Engl. Transl.), 22 (1986) 861. J.H. Kuo, H.U. Anderson, and D.M. Sparlin, J. Solid State Chem., 87 (1990) 55. A. Wold and R.J. Arnott, J. Phys. Chem. Solids, 9 (1959) 176. Y. Takeda, S. Nakai, T. Kojima, R. Kanno, N. Imanishi, G.Q. Shen, O. Yamamoto, M. Mori, C. Asakawa, and T. Abe, Mater. Res. Bull., 26 (1991) 153. M. Verelst, N. Rangavittal, C.N.R. Rao, and A. Rousset, J. Solid State Chem., 104 (1993) 74. M.G. Harwood, Proc. Phys. Soc., 68B (1955) 586. A. Hammouche, E. Siebert, and A. Hammou, Mater. Res. Bull., 24 (1989) 367. K. Kamata, T. Nakajima, T. Hayashi, and T. Nakamura, Mater. Res. Bull., 13 (1978) 49. J.H. Kuo, H.U. Anderson, and D.M. Sparlin, J. Solid State Chem., 83 (1989) 52. J. Kj~er, I.G. Krogh Andersen, N. Mogensen, E. Skou, and H. Boye, in Proceedings of the 14th Riso International Symposium on Materials Science, High Temperature Electrochemical Behaviour of Fast Ion and Mixed Conductors, September 6-10, 1993, Roskilde, Denmark, F.W. Poulsen, J.J. Bentzen, T. Jacobsen, E. Skou, and M.J.L. Osterg&rd (eds.), Risa National Laboratory, Roskilde, Denmark, 1993, p. 281. J.W. Stevenson, M.M. Nasrallah, H.U. Anderson, and D.M. Sparlin, J. Solid State Chem., 102 (1993) 185. R. Ruka, in Proceedings of the Conference on High Temperature Solid Oxide Electrolytes, Vol. 1--Anion Conductors, August 16-17, 1983, Brookhaven National Laboratory, Upton, NY, Report No. BNL 51728, Vol. I, Brookhaven National Laboratory, Upton, NY, 1983, p. 295. J. Mizusaki, H. Tagawa, K. Naraya, and T. Sasamoto, Solid State Ionics, 49 (1991) 111. J.A.M. van Roosmalen and E.H.P. Cordfunke, J. Solid State Chem., 93 (1991) 212.
142
5.42 5.43 5.44 5.45 5.46 5.47 5.48 5.49 5.50 5.51 5.52 5.53 5.54 5.55 5.56 5.57 5.58 5.59 5.60 5.61 5.62 5.63 5.64 5.65 5.66 5.67 5.68 5.69 5.70 5.71
Chapter 5
J.W. Stevenson, M.M. Nasrallah, H.U. Anderson, and D.M. Sparlin, J. Solid State Chem., 102 (1993) 175. M. Ippommatsu, S. Otoshi, H. Sasaki, H. Ohnishi, T. Higuchi, M. Miyayama, and H. Yanagida, J. Mater. Sci., 28 (1993) 4689. H.U. Anderson, see Ref. 5.37, p. 1. P. Kofstad and A. Petrov, see Ref. 5.37, p. 287. A.N. Vlasov and O.O. Butorina, Inorg. Mater. (Engl. Transl.), 29 (1993) 495. J.A.M. van Roosmalen, E.H.P. Cordfunke, R.B. Helmholdt, and H.W. Zandbergen, J. Solid State Chem., 110 (1994) 100. J.A.M. van Roosmalen and E.H.P. Cordfunke, J. Solid State Chem., 110 (1994) 109 and 113. T. Nakamura, G. Petzow, and L.J. Gauckler, Mater. Res. Bull., 14 (1979) 649. Yu.P. Vorob'ev, A.A. Novlev, S.A. Leont'ev, A.N. Men', S.A. Prokudina, and Ya.S. Rubinchik, Inorg. Mater. (Engl. Transl.), 15 (1979) 1142. N. Kamegashira, Y. Miyazaki, and Y. Hiyoshi, Mater. Lett., 2 (1984) 194. O.M. Sreedharan, and M.S. Chandrasekharaiah, J. Mater. Sci., 21 (1986) 2581. M. Lucco Borlera and F. Abbattista, J. Less Common Met., 92 (1983) 55. E.M. Vogel and D.W. Johnson, Thermochim. Acta, 12 (1975) 49. F. Abbattista and M. Lucco Borlera, Ceram. Int., 7 (1981) 137. E. Bergsmark, S. Furuseth, O. Dyrlie, T. Norby, and P. Kofstad, see Ref. 5.19, p. 473. J.B. Goodenough, Phys. Rev., 100 (1955) 564. J.B.A.A. Elemans, B. Van Laar, K.R. Van Der Veen, and B.O. Loopstra, J. Solid State Chem., 3 (1971) 238. G.H. Jonker and J.H. Van Santen, Physica, 16 (1950) 337. E.O. Wollan and W.C. Koehler, Phys. Rev., 100 (1955) 545. J. Tanaka, K. Takahashi, K. Yukino, and S. Horiuchi, Phys. Status Solidi, 80 (1983) 621. T. Hashimoto, N. Ishizawa, N. Mizutani, and M. Kato, J. Mater. Sci., 23 (1988) 1102. H. Taguchi, M. Naga0, and M. Shimada, J. Solid State Chem., 97 (1992) 476. J. Tanaka, M. Umehara, S. Tamura, M. Tsukioka, and S. Ehara, J. Phys. Soc. Jpn., 51 (1982) 1236. R. Koc, H.U. Anderson, and S.A. Howard, see Ref. 5.6, p. 220. R. Koc and H.U. Anderson, J. Mater. Sci., 27 (1992) 5837. J. Palma and C. Pascual, see Ref. 5.19, p. 537. V. Narasimhan, H.V. Keer, and D.K. Chakrabarty, Phys. Status Solidi, 89 (1985) 65. E. Ivers-Tiff6, W. Wersing, M. Schief~l, and H. Greiner, Ber. Bunsenges. Phys. Chem., 94 (1990) 978. E. Ivers-Tiff6, M. Schiel31, H.J. Oel, and W. Wersing, see Ref. 5.37, p. 69. K.Teske, E. Syskakis, and A. Naoumidis, see Ref. 5.37, p. 441.
Cathode
5.72
5.73 5.74 5.75 5.76 5.77 5.78 5.79 5.80 5.81
5.82 5.83 5.84 5.85 5.86 5.87 5.88 5.89 5.90 5.91
5.92 5.93
143
A. Mackor, C.I.M.A. Spee, E.A. van der Zouwen-Assink, J.L. Baptista, and J. Schoonman, in Proceedings of the 25th IECEC, August 12-17, 1990, Reno, NV, Vol. 3, American Institute of Chemical Engineers, New York, 1990, p. 251. P.K. Gallagher, D.W. Johnson, Jr., and E.M. Vogel, J. Am. Ceram. Soc., 60 (1977) 28. V.I. Pavlov, A.K. Bogush, and G.L. Bychkov, Inorg. Mater. (Engl. Transl.), 20 (1984) 752. A. Mackor, T.P.M. Koster, J.G. Kraaijkamp, J. Gerretsen, and J.P.G.M. van Eijk, see Ref. 5.19, p. 463. E.M. Vogel and D.W. Johnson, Thermochim. Acta, 12 (1975) 49. R.J.H. Voorhoeve, J.P. Remeika, L.E. Trimble, A.S. Cooper, F.J. Disalvo, and P.K. Gallagher, J. Solid State Chem., 14 (1975) 395. R. Hildrum, S. Aasland, and 0. Johannesen, Solid State Ionics, 66 (1993) 207. G.H. Jonker, Physica (Amsterdam), 20 (1954) 1118. M. Kertesz, I. Riess, D.S. Tannhauser, R. Langpape, and F.J. Rohr, J. Solid State Chem., 42 (1982) 125. K. Katayama, T. Ishihara, H. Ohta, S. Takeuchi, Y. Esaki, and E. Inukai, J. Ceram. Soc. Jpn. (Nippon Seramikkusu Kyokai Gakujutsu Ronbunshi), 97 (1989) 1327. S. Otoshi, H. Sasaki, H. Ohnishi, M. Hase, K. Ishimaru, M. Ippommatsu, T. Higuchi, M. Miyayama, and H. Yanagida, J. Electrochem. Soc., 138 (1991) 1519. A. Hammouche, E.L. Schouler, and M. Henault, Solid State Ionics, 28-30 (1988) 1205. H. Lauret, E. Caignol, and A. Hammou, see Ref. 5.19, p. 479. J.A.M. van Roosmalen, J.P.P. Huij