Studies in Surface Science and Catalysis 105 PROGRESS IN ZEOLITE AND MICROPOROUS MATERIALS
Studies in Surface Science and Catalysis 105 PROGRESS IN ZEOLITE AND MICROPOROUS MATERIALS
This Page Intentionally Left Blank
Studies in Surface Science and Catalysis A d v i s o r y E d i t o r s : B. D e l m o n a n d J.T. Yates Vol. 105
PROGRESS IN ZEOLITE AND MICROPOROUS MATERIALS
PART A Proceedings ofthe 1lth International Zeolite Conference, Seoul, Korea, August 12-17, 1996 Editors HakzeChon Son-Ki Ihm Korea Advanced Institute of Science and Technology, Taejon, Korea
Young Sun Uh
Korea Institute of Technology, Seoul, Korea
1997 ELSEVIER Amsterdam -- Lausanne -- New York-- Oxford -- Shannon -- Tokyo
ELSEVIER SCIENCE B.V. Sara Burgerhartstraat 25 P.O. Box 211, 1000 AE Amsterdam, The Netherlands
ISBN 0-444'82344-1 © 1997 Elsevier Science B.V. All rights reserved. No part of this publication may be reproduced, stored in a retrieval system or transmitted in any form or by any means, electronic, mechanical, photocopying, recording or otherwise, without the prior written permission of the publisher, Elsevier Science B.V., Copyright & Permissions Department, P.O. Box 521, 1000 AM Amsterdam, The Netherlands. Special regulations for readers in the U.S.A. - This publication has been registered with the Copyright Clearance Center Inc. (CCC), 222 Rosewood Drive, Danvers, MA 01923. Information can be obtained from the CCC about conditions under which photocopies of parts of this publication may be made in the U.S.A. All other copyright questions, including photocopying outside of the U.S.A., should be referred to the copyright owner, Elsevier Science B.V., unless otherwise specified. No responsibility is assumed by the publisher for any injury and/or damage to persons or property as a matter of products liability, negligence or otherwise, or from any use or operation of any methods, products, instructions or ideas contained in the material herein. This book is printed on acid-free paper. Printed in The Netherlands
Contents Part A xxxi
Preface Organizing Committee of the 11th IZC
XXXII1
International Advisory Board to the 1lth IZC
xxxvi
Financial Supports
xxxix
I. Synthesis Directed Synthesis of Organic/Inorganic Composite Structures G.D. Stucky, Q. Huo, A. Firouzi, B.F. Chmelka, S. Schacht, I.G. VoigtMartin and F. Schiith Incorporation and Stability of Trivalent Cations in Mesoporous Silicas Prepared Using Primary Amines as Surfactant S. Gontier and A. Tuel
29
Synthesis ofLamellar Aluminophosphates via the Supramolecular Templating Mechanism A. Sayari
37
Synthesis and Hydrothermal Stability of a Disordered Mesoporous Molecular Sieve R. Ryoo, J.M. Kim, C.H. Shin and J. Y. Lee
45
Preparation of Silica-Pillared Molecular Sieves from Layered Silicates S.-Y. Jeong, O.-E Kwon, J.-K. Sub, H. Jin and J.-M. Lee
53
A New Synthetic Route and Catalytic Characteristics of Pillared Rectorite Molecular Sieves J. Guan, Z Yu, Z Chen, L. Tang and X. Wang
61
Textural Control ofMCM-41 Aluminosilicates F. Di Renzo, N. Coustel, M. Mendiboure, H. Cambon and F. Fajula
69
New Routes for Synthesizing Mesoporous Material Y. Sun, W. Lin, £ Chen, Y. Yue and W. Pang
77
Synthesis and Characterization ofFeSiMCM-41 and LaSiMCM-41 N.-Y. He, S.-L. Bao and Q.-H. Xu
85
Synthesis of Titanium-Containing Mesoporous Molecular Sieves with a Cubic Structure K.A. Koyano and T. Tatsumi
93
Short Range Order of MCM-41 and Mesostructured Aluminiumphosphate C. Pophal, R. Schnell and H. Fuess
101
Syntheses ofMesoporous Aluminosilicates from Layered Silicates Containing Aluminum S. lnagaki, Y. Yamada and Y. Fukushima
109
Structure Descriptors for Organic Templates Employed in Zeolite Synthesis R.E. Boyett, A.P. Stevens, M.G. Ford and P.A. Cox
117
Quantitative Aspects in the Crystallization of Zeolites H. Lechert, T. Lindner and P. Staelin
125
A Computational 'Expert System' Approach to Design Synthesis Routes for Zeolite Catalysts T. Selvam, D.N. lyer, R.C. Deka, A. Chatterjee and R. Vetrivel
133
A New Method for Enhancing Zeolite Crystallization by Using Oxyacids/Salts of Group VA and VIIA Elements as Promoters A. Bhaumik, A.A. Belhekar and R. Kumar
141
The Influence of Mixed Organic Additives on the Zeolites A and X Crystal Growth V.P. Petranovskii, Y. Kiyozumi, N. Kikuchi, H. Hayamisu, Y. Sugi and F. Mizukami
149
Studies of the Crystallization of ZSM-5 under High Gravitational Force Field W.J. Kim, D.T. Hayhurst, S.A. Lee, 3/1.C. Lee, C. IV..Lira and J.C. Yoo
157
vii Structure Directing Role ofNa ÷ and TMA + Cations in 18-Crown-6 Ether Mediated Crystallization of EMT, MAZ and SOD Aluminosilicate Zeolites E.J.P. Feijen, B. Matthijs, P.J. Grobet, J.A. Martens and P.A. Jacobs
165
Synthesis of High-Silica FAU-,EMT-,RHO- and KFI-Type Zeolites in the Presence of 18-Crown-6 Ether T. Chatelain, J. Patarin, E. Brendl~, F. Doughier, J.L. Guth and P. Schulz
173
Synthesis of Zeolites in a Microwave Heating Environment J.P. Zhao, C. Cundy and J. Dwyer
181
Synthesis of Octahedral Molecular Sieves C.-L. O'Young and S.L. Suib
189
Syntheses and Crystal Structures of Two "Organozeolites" K. Maeda, J. Akimoto, Y. Kiyozumi and F. Mizukami
197
ERS-8: A New Class of Microporous Aluminosilicates G. Perego, R. Millini, C. Perego, A. CaratL G. Pazzuconi and G. Bellussi
205
Synthesis and Characterization of Levyne Type Zeolite Obtained from Gels with Different SiO2/Al203Ratios C.V. Tuoto, J.B. Nagy and A. Nastro
213
Synthesis ofETS-10 Molecular Sieve from Systems Containing TAABr Salts P. De Luca and A. Nastro
221
Synthetic Clinoptilolite and Distribution of Aluminum Atoms in the Framework of liEU Type Zeolites M. Kato, S. Satokawa and K. ltabashi
229
Preparation of Ultramarine Analogs from Zeolites S. Kowalak, M. Str6zyk, M. Pawlowska, M. Miluska and J. Kania
237
Exploration of Non Conventional Routes to Synthesize MFI Type Titanoand (Boro-Titano)- Zeolites M. Shibata, J. G~rard and Z Gabelica
245
Synthesis, Characterization and Catalytic Properties of Vanadium Containing VPI-5 K. Chaudhari, T.Kr. Das, A.J. Chandwadkar, J.G. Chandwadkar and S. Sivasanker
253
viii Crystallization of Titanium Silicalite-1 from Gels Containing Hexanediamine and Tetrapropylarrm,onium Bromide A. Tuel
261
Synthesis and Characterisation of Gallium and Germanium Containing Sodalites G.M. Johnson and M. T. Weller
269
Synthesis and Characterization of Chromo, Ferro, Mangano and Vanadio Silicates with MTW Structure M.L.S. Corrda, M. Wallau and U. Schuchardt
277
Improved Synthesis of (Ga)- and (Ga, Al)- Faujasites Z. Gabelica, K Norberg and T. Ito
285
A Study on the Crystallization of Binderless Zeolite X X. Luo, X.. He and J. Shen
293
Synthesis of Large Crystals of Molecular Sieves-A Review S. Qiu, W. Pang and R. Xu
301
Synthesis and Characterization of ZSM-5 in Fluoride Medium: The Role of NH4+ and K ÷ Cations E. Nigro, R. Mostowicz, F. Crea, F. Testa, R. Aiello and J.B. Nagy
309
Three-Dimensional Real-Time Observation of Growth and Dissolution of Silicalite Crystal A. lwasaki, L Kudo and T. Sano
317
Synthesis of Mordenite and ZSM-11 Zeolites from Very Dense Systems" Formation of Self-Bonded Pellets P. De Luca, F. Crea, R. Aiello, A. Fonseca and J.B. Nagy
325
Studies on Crystallization of ZSM-12 Type Zeolite A. V. Toktarev and K. G. lone
333
Synthesis of Nanocrystalline Zeolite Beta in the Absence of Alkali Metal Cations M.A. Camblor, A. Corma, A. Mifsud, J. P~rez-Pariente and S. Valencia
341
Synthesis of Zeolite Beta with Low Template Content M. W.N. C. Carvalho and D. Cardoso
349
Synthesis and Characterization of Sn- Containing ZSM-48 Type Molecular Sieves Using Different Templates N.K. Mal, V. Ramaswamy, B. Rakshe and A. V. Ramaswamy
357
Inorganic Cations in AIPO4 Synthesis E. Halvorsen, A. Karlsson, T. Haug, D. Akporiaye and K.P. Lillerud
365
New Insights into the Study oflndiumphosphate Molecular Sieves L.L. Koh, Y. Xu, H. Du and W. Pang
373
Synthesis and Characterization of Novel Open-Framework Cobalt Phosphates from Aqueous-Alcoholic Systems J. Yu, Q. Gao, J. Chen and R. Xu
381
A Family of Unusual Lamellar Aluminophosphates Synthesized from NonAqueous Systems Q. Gao, J. Chen, S. Li and R. Xu
389
Synthesis of Various Indium Phosphates in the Presence of Amine Templates H. Du, J. Chen and W. Pang
397
Steric-Electronic Model of Templating Effect Z. Liu and R. Xu
405
II. Characterization The Synthesis and Characterization ofUTD-I: The First Large Pore Zeolite Based on a 14 Membered Ring System K.J. Balkus Jr., M. Biscotto and A. G. Gabrielov
415
The Nature of the Acid Sites in Mesoporous MCM-41 Molecular Sieves A. Liepold, K. Roos, W. Reschetilowski, R. Schmidt, M. StOcker, A. Philippou, M. W. Anderson, A.P. Esculcas and J. Rocha
423
Solid Mesoporous Base Catalysts Comprising ofMCM-41 Supported Intraporous Cesium Oxide K.R. Kloetstra and H. van Bekkum
431
Non-Framework Aluminium in Highly Dealuminated Y Zeolites Generated by Steaming or Substitution W. Lutz, E. LOftier, M. Fechtelkord, E. Schreier and R. Bertram
439
Spectroscopic Studies of a Magnesium Substituted Microporous Aluminophosphate DAF- 1 S.J. Thomson and R.F. Howe
447
MASNMR Chemical Shit, s and Structure in Frameworks M.T. Weller, S.E. Dann, G.M. Johnson and P.J. Mead
455
A New Method for the NMR-Spectroscopic Measurement of the Deprotonation Energy of Surface Hydroxyl Groups in Zeolites E. Brunner, J. Ka'rger, M. Koch, H. Pfeifer, H. SachsenrOder and B. Staudte
463
~70 NMR Studies of Siliceous Faujasite L.M. Bull andA.K. Cheetham
471
Deuteron Magnetic Resonance Studies of Ammonia in AgNaY-Zeolites M. Hartmann and B. Boddenberg
479
Spectroscopic Studies of 170 and 180 Labelled ZSM-5 Zeolites F. Bauer, H. Ernst, E. Geidel, Ch. Peuker and W. Pilz
487
Anisotropic Motion of Water in Zeolites EMT, L and ZSM-5 as Studied by D- and H-NMR Line Splitting A. Wingen, W.D. Basler and H. Lechert
495
EXAFS and NMR Studies of the Incorporation of Zn(II) and Co(II) Cations into Tetrahedral Framework Sites of AIPO4 Molecular Sieves N.N. Tusar, A. Tuel, 1. Arcon, A. Kodre and K Kaucic
501
Si, AI Solid Solution in Sodalite: Synthesis, 298i NMR and X-Ray Structure M. Sato, E. Kojima, H. Uehara and M. Miyake
509
Substitution of Silicon and Metal Ions in Small Pore Aluminophosphate Molecular Sieves with Chabazite Structure: Synthesis and MASNMR Study D.K. Chakrabarty, S. Ashtekar, A.M. Prakash and S. K K Chilukuri
517
Inclusion of Sodium Chloride in Zeolite NaY Studied by 23NaNMR Spectroscopy U. Tracht, A. Seidel and B. Boddenberg
525
Spectroscopic Investigation of the State of Aluminium in MCM-41 Aluminosilicates S. Viale, E. Garrone, F. Di Renzo, B. Chiche and F. Fajula
533
Boiling-Point Elevation of Water Confined in Mesoporous MCM-41 Materials Probed by 1H NMR E.W. Hansen, R. Schmidt and M. StOcker
543
In Situ Studies of Catalytic Reactions in Zeolites by Means of PFG and MAS NMR Techniques J. Karger and D. Freude
551
Vibrational Study of Benzene Adsorbed in NaY Zeolite by Neutron Spectroscopy H. Jobic and A.N. Fitch
559
Infrared Holeburning Spectroscopy in Acid Zeolites M. Bonn, M.J.P. Brugmans, H.J. Bakker, A.W. Kleyn and R.A. van Santen
567
Exploring the Sites of Adsorbed Pyrrolidine Derivatives in Y Zeolites by Joined Infrared Spectroscopic and Computer Simulation Studies E. Geidel, K. Krause, J. Kindler and H. FOrster
575
Preparation and Characterisation of Ru-Exchanged NaY Zeolite: An Infrared Study of CO Adsorption at Low Temperatures S. Wrabetz, U. Guntow, R. SchlOgl and H. G. Karge
583
New Insight into the Mechanism of Zeolite Catalyzed Nucleophilic Amination Via In Situ Infrared Spectroscopy C. Griindling, V.A. Veefkind, G. Eder-Mirth and J.A. Lercher
591
Coke Formation in Zeolites Studied by a New Technique: Ultraviolet Resonance Raman Spectroscopy C. Li and P. C. Stair
599
Preparation of Titanium-Containing Large Pore Molecular Sieve from H-AIBeta Zeolite X. Guo, X. Wang, G. Wang and G. Li
607
Syntheses and Raman Spectroscopic Study of Bis- and Tris-(1,10Phenanthroline) Manganese(II) Complexes Encapsulated in Faujasite-Y B. Zhan and X. Li
615
Chemometric Analysis of Diffuse Reflectance Spectra of CoA Zeolites: Spectroscopic Fingerprinting of Co2+-Sites A.A. Verberckmoes, B.M. Weckhuysen and R.A. Schoonheydt
623
xii Raman Characterization of the Selenium Species Formed inside the Confined Spaces of Zeolites V. V. Poborchii
631
Determination of Basic Site Location and Strength in Alkali Exchanged Zeolites D. Murphy, P. Massiani, R. Franck and D. Barthomeuf
639
A Spectroscopic Study of the Initial Stage in the Crystallization of TPASilicalite-1 from Clear Solutions B.J. Schoeman
647
Characterization and Catalytic Properties of the Galliumphosphate Molecular Sieve Cloverite R. Fricke, M. Richter, H.-L. Zubowa and E. Schreier
655
Preparation of Titanosilicate with Mordenite Structure by Atom-planting Method and Its Catalytic Properties for Hydroxylation of Aromatics P. Wu, T. Komatsu and T. Yashima
663
Characterization of Zeolite Basicity Using Iodine as a Molecular Probe S.Y. ChoL Y. S. Park and K.-B. Yoon
671
Ship-in-Bottle Synthesis of Pt and Ru Carbonyl Clusters in NaY Zeolite Micropore and Ordered Mesoporous Channels ofFSM-16; XAFS/FTIR/TPD Characterization and Their Catalytic Behaviors M. Ichikawa, T. Yamamoto, W. Pan and T. Shido
679
Characterization and Reactivity ofNi,Mo-Supported MCM-41 Catalysts for Hydrodesulfurization J. Cui, E-H. Yue, E Sun, W. -Y. Dong and Z Gao
687
Probing the Hydrophobic Properites of MCM-41-Type Materials by the Hydrophobicity Index R. Glaser, R. Roesky, T. Boger, G. Eigenberger, S. Ernst and J. Weitkamp
695
Characterisation of Acid- Base- and Redox- Type Sites in ZSM-5 Zeolites by Sorption Rate "Spectroscopy" Gy. Onyesty6k, J. Valyon and L. V. C. Rees
703
A Picosecond Spectroscopic Study on the Proton Transfers of 6Hydroxyquinoline in Zeolite Cages H. Yu, J. Park, N.W. Song and D.-J. Jang
711
xiii Ethylene Dimerization in Nickel Containing SAPO Materials Studied by Electron Spin Resonance and Gas Chromatography: - Influence of the Channel Size M. Hartmann and L. Kevan
717
The Electronegativity Equalization Method(EEM) as a Promising Tool for the Analysis of Zeolite Catalyzed Reactions G.O.A. Janssens, H. Toufar, B.G. Baekelandt, W.J. Mortier and R.A. Schoonheydt
725
Synthesis and Characterization of Iron Modified L-Type Zeolite Y.S. Ko, W.S. Ahn, J.H. Chae and S.HMoon
733
Synthesis, Characterization and Catalytic Properties of VS-2 H. Du, G. Liu, Z. Da and E. Min
741
Preparation and Characterization of Manganese Bipyridine Complexes in Zeolites with Different Pore Architectures S. Ernst and B. Jean
747
Metal Substituted ATS Aluminophosphate Molecular Sieves D. Akolekar and R.F. Howe
755
The Modified Hydrophobicity Index as a Novel Method for Characterizing the Surface Properties of Titanium Silicalites J. Weitkamp, S. Ernst, E. Roland and G. F. Thiele
763
The Thermal Stability of GaUophosphate Cloverite W. Schmidt, F. Schiith and S. Kallus
771
Electron Spin Resonance Studies of 02" Adsorbed on Aluminophosphate Molecular Sieves S.B. Hong, S.J. Kim, Y.-S. Choi and Y.S. Uh
779
The Affinity Order of Organics on Hydrophobic Zeolite Silicalite-1 Studied by Thermal Analysis Y. Long, H. Jiang and H. Zeng
787
Chemistry of CoAPO-11 and VAPO-5" ESR Studies of Molecular Oxygen Adducts C. Naccache, M. Vishnetskaya and K.J. Chao
795
Cupric Ion Species in Cu(II)-Exchanged Gallosilicate K-L and Comparison with Aluminosilicate K-L J.-S. Yu, S.B. Hong and L. Kevan
801
xiv
Part B 111. Catalysis - First Part Structure-Reactivity-SelectivityRelationships in Reaction of Organics over Zeolite Catalysts P.B. Venuto
811
Conversion of Propan-2-01 on Zeolite LaNaY Investigated by in situ M A S
853
Structure and Catalytic Activity of Co-Based Bimetallic Systems in NaY Zeolite: Low Temperature Methane Activation L. Guczi, Z. Koppany, K. V. Sarma, L. Borkd and I. Kiricsi
86 1
The Aromatization of Methane over MokIZSM-5 Zeolites without Using Oxidants M. Xie, X Yang, W. Chen, L. Tao, X Wang, G. Xu, L. Wang, Y.-D. Xu,S.Liu andX-X Guo
869
Properties of PtSn/KL Catalysts for n-Hexane Aromatization J.H. Chae and S.H. Moon
877
A New Process of Light Naphtha Aromatization Using a Zeolite-Based Catalyst with Long-Time Stability S.Fukase, N Igarashi, K. Aimoto, H. Inoue and H. On0
885
Preparation of Zeolites Incorporating Molybdenum Sulfide Clusters with Unusual Carbon Number Distribution in c 0 - H ~ Reactions M. Taniguchi, Y. Ishii, T. Murata, M. Hidai and T. Tatsumi
893
CO Hydrogenation over Pd/HZSM-5 Catalysts: Temperature-Programmed Desorption, 13CO/C180Isotope Analysis, and in-situ Infrared Spectroscopy S.-K. Ihm, J-K. Jeon and D.-K. Lee
901
Reaction Mechanisms of Heptane Isomerization and Cracking on BifunctionalPt/H-Beta Zeolites E. Blomsma. LA. Martens and P.A. Jacobs
909
NMR Spectroscopy under Continuous-Flow Conditions M. Hunger, T.Horvath andJ Weitkump
XV
Pt/Zeolite Catalysts for Hydrocracking: A Comparative Study on FAU and EMT K Zholobenko, A. Garforth, F. Bachelin and J. Dwyer
917
Acidity in Working Zeolites: Use of a Stabilised Carbenium in a New Route for the Synthesis of Secondary Amides on ZSM-5 F. Thibault-Starzyk, M.M. Bettahar, J. Saussey and J.-C. Lavalley
925
Temperature Effects on Deactivation Rate and on Nature of Coke Formed from Propene over Mordenites C.A. Henriques, J.C. Afonso, P. Magnoux, M. Guisnet and J.L.F. Monteiro
933
Catalytic Degradation of High Density Polyethylene by HZSM-5 Zeolite KJ. Fernandes Jr., A.S. Araftjo and G.J.T. Fernandes
941
The Use of Cyclohexanol Dehydration, Isobutane Cracking and 2,6-DIPN Synthesis over Dealuminated Mordenite to Probe Acidity A.W. O'Donovan and C.T. O'Connor
949
Characterization and Reactivity Study of Rhenium-Impregnated Zeolite Y Catalysed Metathesis of Olefins H. Hamdan and Z. Ramli
957
Propene Oligomerization over Dealuminated Mordenite 1. Gigstad and S. Kolboe
965
The Induction Period in Ethylbenzene Disproportionation over Large Pore Zeolites U. Weifl, M. Weihe, 3/1. Hunger, H.G. Karge and J. Weitkamp
973
Effect of Ga on the Hydrogen Transfer Activity of Zeolites with the Offretite Structure P.-S.E. Dai, C.M. Tsang, R.H. Petty, M.. Somervell, B. Williamson andM.L. Occelli
981
TPR and XPS Studies of Iron-Exchanged Y Zeolites and Their Activity during Dibenzothiophene Hydrodesulfurization M.. Nagai, O. Uchino, J. Okubo and S. Omi
989
Hydroconversion of Aromatics on Metal-Zeolite Catalysts L.P. Poslovina, V.G. Stepanov, L. V. Malysheva, E.A. Paukshtis, L.A. Vostrikova and K. G. lone
997
xvi Low Temperature Hydrocracking of Paraffinic Hydrocarbons over Hybrid Catalysts 1. Nakamura, K. Sunada and K. Fufimoto
1005
A Comparative Study of Titanium-Containing Aluminophosphate Molecular Sieves TAPO-5, TAPO-11 and TAPO-36 M.H. Zahedi-Niaki, P.N. Joshi and S. Kaliaguine
1013
MCM-41-Type Molecular Sieves as Carriers for Metal-Phthalocyanine Complexes S. Ernst, R. Glaser andM. Selle
1021
Application of CoAPO-5 Molecular Sieves as Heterogeneous Catalysts in Liquid Phase Oxidation of Alkenes with Dioxygen H.F. ~ J . van Breukelen, M.E. Gerritsen, KM. Ummels, J.S. Broens and J.H. C. van Hooff
1029
Selective Oxidation of Aromatic Hydrocarbons over Copper Complexes Encapsulated in Molecular Sieves R. Raja and P. Ratnasamy
1037
Cation Effects in the Oxidation of Adsorbed Cyclohexane in Y Zeolite: An in situ IR Study D.L. Vanoppen, D.E. De Vos and P.A. Jacobs
1045
Influence of Extra-Framework Alumina in H-[AI]ZSM-5 Zeolite on the Direct Hydroxylation of Benzene to Phenol J.L. Motz, H. Heinichen and W.F. HOlderich
1053
The Stability of Chromium in Chromium Molecular Sieves under the Conditions of Liquid Phase Oxidations with tert-Butyl Hydroperoxide H.E.B. Lempers and R.A. Sheldon
1061
Oxidation of Olefins and Alkanes with Various Peroxides, Catalyzed by Triamine Containing Manganese Faujasites D.E. De Vos, J.L. Meinershagen and T. Bein
1069
Characterization and Reversible Reduction/Oxidation of Zeolite-Hosted Tiand V-Oxide Dispersions G. Grubert, M. Wark, W. Griinert, M. Koch and G. Schulz-Ekloff
1077
Zirconium Containing Mesoporous Silicas: New Catalysts for Oxidation Reactions in the Liquid Phase S. Gontier and A. Tuel
1085
xvii Synthesis of Aluminium Free Titanium Silicate with the BEA Structure Using a New and Selective Template and Its Use as a Catalyst in Epoxidations J.C. van der Waal, P. Lin, M.S. Rigutto and H. van Bekkum
1093
Incorporation of Vanadium into ZSM-5, Mordenite and Y Type Zeolite and Their Catalytic Properties G.-J. Kim, J.-H. Kim and H. Shoji
1101
Catalytic Tuning of the Olefin Epoxidation with Hydrogen Peroxide and Faujasite Y Occluded Mn Bipyridine Complexes P.-P. Knops-Gerrits, H. Toufar and P.A. dacobs
1109
The Selective Oxidation of Cyclohexane Using Iron(Ill) Incorporated Zeolite Y and Iron(III) Supported Zeolite Y in a Heterogeneous Biomimetic Oxidation System C.-H. Park, S.-S. Nam, S.B. Kim, S.-B. Kim, K.-W. Jun and K.-I4(. Lee
1117
Solid Catalysts for the Hydroxyalkylation of Aromatics with Epoxides. Intermolecular Hydroxyalkylation versus Intramolecular Hydroxyalkylation ~A. Elings, R.S. Downing and R.A. Sheldon
1125
Heterogeneously-Catalyzed Hydroalkoxylation of Limonene and alphaPinene in the Presence of Beta Zeolite K. Hensen, C. Mahaim and I~.F. HOlderich
1133
Photochemistry of Alkyl Ketones Included within the Zeolite Cavities: The Effect of Ion-exchanged Alkali Metal Cations and Types of Zeolites H. Yamashita, N. Sato, M. Anpo, T. Nakafima, M. Hada and H. Nakatsufi
1141
Acylation of Phenol with Acetic Acid. Effect of Density and Strength of Acid Sites on the Properties ofMFI Metallosilicates F. Jayat, M. Guisnet, M. Goldwasser and G. Giannetto
1149
Structural Design for Y-type Zeolite on Large Molecule Conversion. Alkylation of Phenol with Long Chain Olefin. X-W.. Li, M. Han, X.-Y. Liu, Z.-F. Pei and L. She
1157
Zeolite-Catalysed Rearrangement of lsophorone Oxide J.A. Elings, H.E.B. Lempers and R.A. Sheldon
1165
Vapour-Phase Beckmann Rearrangement Using B-MFI Zeolites J. ROseler, G. Heitmann and I'EF. HOlderich
1173
xviii Catalytic Properties of Fluorinated CeY S. Kowalak, M. Laniecki, M. Pawlowska, K.£ Balkus Jr. and A. Khanmamedova
1181
Evaluation of Catalyst Deactivation on Beckmann Rearrangement over Indiosilicate Modified with Noble Metals M.N.A. Nasution, T. Takahashi and T. Kai
1189
Selective Fries Rearrangement of Phenyl Acetate into Hydroxy Acetophenones Catalyzed by High-Silica Zeolite NCL-1 M. Sasidharan and R. Kumar
1197
Selective Hydrogenation of Cinnamaldehyde to Cinnamyl Alcohol on LZeolite Supported Catalysts G. LL T. Li, Y.-D. Xu, S. Wong and X.-X Guo
1203
Zeolite Catalysts for the Friedel-Craffs Alkylation of Methyl Benzoate, a Strongly Deactivated Aromatic Substrate B. Janssens, P. Carry, R. Claessens, G. Baron and P.A. Jacobs
1211
Methanol Amination over Small-Pore Zeolite Catalysts K. Segawa and M. C. Ilao
1219
Synthesis of Aniline from Phenol and Ammonia over Zeolite Beta N. Katada, S. lo'ima, H. lgi and M. Niwa
1227
Cyclodimerization ofBicyclo[2.2.1 ]Hepta-2,5-Diene in the Presence of Rhodium-Containing Zeolite Catalysts N.F. Goldshleger, B.L Azbel, Ya.I. Isakov, E.S. Shpiro and Kh.M. Minachev
1235
Vinyl Chloride Synthesis on Zeolite Catalysts: The Role of Strong Lewis Acid-Base Pair Sites E.B. Uvarova, L.M. Kustov, I.L Lishchiner, O.V. Malova and V.B. Kazansky
1243
IV. C a t a l y s i s - S e c o n d P a r t
Influence of Zeolite Pore Structure on Catalytic Reactivity A. van de Runstraat, P.£ Stobbelaar, J. van Grondelle, B.G. Anderson, L.£ van IJzendoorn and R.A. van Santen
1253
xix Regio Selectivity in the Hydrogenation of Geraniol over Platinum Containing Zeolites D. Tas, R.F. Parton, K. Vercruysse and P.A. Jacobs
1261
Zeolite Catalyzed Regioselective Synthesis of lndoles P.J. Kunkeler, M.S. Rigutto, R.S. Downing, H.J.A. de Vries and H. van Bekkum
1269
Shape-Selective Zeolite Catalysed Synthesis of Monoglycerides by Esterification of Fatty Acids with Glycerol E. Heykants, W.H. Verrelst, R.F. Parton and P.A. Jacobs
1277
Selective Key-Lock Catalysis in Dimethylbranching of Alkanes on TON Type Zeolites W. Souverijns, J.A. Martens, L. Uytterhoeven, G.F. Froment and P.A. Jacobs
1285
Kinetics Study ofEthylbenzene Disproportionation with Medium and Large Pore Zeolites N. Arsenova, W.O. Haag and H. G. Karge
1293
Application of a Kinetic Model for Investigation of Aromatization Reactions of Light Paraffins and Olefins over HZSM-5 D.B. Lukyanov
1301
Conversion of n-Pentane to Benzene Toluene and para-Xylene over Pore Size Controlled Ga203 Incorporated ZSM-5 Zeolite KS. Bhat, J. Das and A.B. Halgeri
1309
The Influence of Reagents on Shape-Selective Alkylation of Biphenyls over H-Mordenite M. Matsumoto, X. Tu, T. Matsuzaki, T. Hanaoka, E Kubota, E Sugi, J.-H. Kim, K. Nakajima, A. Igarashi and K. Kunimori
1317
Selective Benzene Isopropylation over Fe-Containing Zeolite Beta A.V. Smirnov, F. Di Renzo, O.E. Lebedeva, D. Brunel, B. Chiche, A. Tavolaro, B.V. Romanovsky, G. Giordano, F. Fajula and 1.1. Ivanova
1325
Para-Selective Gas Phase 02 Oxidations of Alkylaromatics over CVD Fe/Mo/Borosilicate Molecular Sieve J.S. Yoo, P.S. Lin and S.D. Elfline
1333
A Model Study on Zeolite Composites for Improved Catalyst Selectivity N. van der Pull, LB. Janto-Saputro, H. van Bekkum and J.C. Jansen
1341
XX
Toluene Disproportionation over ZSM-5 Catalysts Covered with Silicalite Shell C.S. Lee, T.-J. Park and IE.Y. Lee
1349
Ethylation of Ethylbenzene to Produce para-Diethylbenzene X. Wang, G. Wang, H. Guo and X. Wang
1357
Mechanisms of the Skeletal Isomerization of n-Butene over a HFER Zeolite. Influence of Coke Deposits. M. Guisnet, P. Andy, N.S. Gnep, C. Travers and E. Benazzi
1365
Reaction of n-Butene over H-ZSM-5 Zeolite. Influence of the Acid Strength on the Isobutene Selectivity P. M&iaudeau, T. Vu. Anh, H. Le Ngoc and C. Naccache
1373
Skeleton Hydroisomerization ofHexene-1 in the Presence of Synthesis Gas on Zn-Cr/HZSM-5 Catalyst V.M. Mysov, V.G. Stepanov and K. G. lone
1381
Skeletal Isomerization of 1-Butene over Zeolite Catalysts: A Computational Study R. Millini and S. Rossini
1389
Studies of Crystallization of SAPO-11 Molecular Sieve and Applications for Catalytic Skeletal Isomerization of Linear Butylenes H. Tian and C. Li
1397
Pt-Cu Bimetallics in H-Y Zeolite: Microcalorimetric Study of the Effect of Copper on the Catalyst Acidity A. Auroux, Y. Ben Taarit, M. Lokolo, P. Meriaudeau and C. Naccache
1405
La-EMT, a Promising Catalyst for Isobutane/2-Butene Alkylation H. Mostad, M. StOcker, A. Karlsson, H. Junggreen and B. Hustad
1413
Skeletal Isomerization of n-Butenes on Modified ZSM-35 Catalysts B.S. Kwak, J.H. Jeong and S.H. Park
1423
Selectivity to the Skeletal Isomerization of 1-Butene over Ferrierite(FER) and ZSM-5 (MFI) Zeolites G. Seo, H.S. Jeong, J.M. Lee and B.J. Ahn
1431
xxi
V. Environment High Potential of Novel Zeolitic Materials as Catalysts for Solving Energy and Environmental Problems T. Inui
1441
Modification and Stabilization of Cu-ZSM-5 by Introduction of a Second Cation A. V. Kucherov, C.P. Hubbard, T.N. Kucherova and M. Shelef
1469
Reactivity of Adsorbates in the Decomposition of Nitric Oxide over CuZSM-5 Catalysts S.S. C. Chuang and B. Lopez
1477
Quantum Chemical Investigation of Reactants in Selective Reduction of NOx on Ion Exchanged ZSM-5 M. Yamadaya, H. Himei, T. Kanougi, E Oumi, M. Kubo, A. Stir#ng, R. Vetrivel, E. Broclawik and A. Miyamoto
1485
The Role of Water for NO Reduction by Hydrocarbons over Copper IonExchanged Mordenite Type Zeolite Catalysts M.H. Kim, I.-S. Nam and E G. Kim
1493
Catalytic Reduction of Nitrogen Monoxide by Methane over Pd-Loaded ZSM-5 Zeolites. Roles of Acidity and Pd Dispersion M. Misono, Y. Nishizaka, M. Kawamoto and H. Kato
1501
Zeolites in the Environmental Protection - Decomposition of Chlorofluorocarbons over Zeolite Catalysts Z. K6nya, L Hannus and 1. Kiricsi
1509
Preparation of Cu-Na-ZSM-5 Catalysts by Thermal Spreading Techniques W. Griinert, T. Liese and C. Schobel
1517
Preparation, Characterization and Catalytic Activity Towards Lean NOx Reduction of Over-exchanged Cu-ZSM-5 Catalysts G. Moretti, G. Minelli, P. Porta, P. Ciambelli, P. Corbo, M.. Gambino, F. Migliardini and S. Iacoponi
1525
Factors Controlling Catalytic Activity of H-Form Zeolites for the Selective Reduction of NO with CI-L A. Satsuma, M. Iwase, A. Shichi, T. Hattori and Y. Murakami
1533
xxii CO Oxidation and NO Reduction by CO on Differently Prepared CuO/Mordenites K.-H. Lee and B.-H. Ha
1541
Steam Deactivation of Transition Metal MFI Zeolite Catalysts for NOx Reduction P. Budi, E. Curry-Hyde and R.F. Howe
1549
ln-situ IR Studies of Surface Species during the Selective Catalytic Reduction(SCR) of NO by Propene over Cu-ZSM-5 Zeolites D.H. Kim, I.C. Hwang and S.I. Woo
1557
Reduction of NO by CO Using a Zeolite Catalyst Obtained from Fly Ash E. L6pez-Sa#nas, P. Salas, L Schifter, M. Mor6n, S. Castillo and E. Mogica
1565
ln-situ FT-IR and Catalytic Studies of the Selective Reduction of Nitric Oxide by Carbon Monoxide over Au/NaY Catalysts: Effect of Adding Hydrogen to the Reaction Gas Mixture T.M. Salama, R. Ohnishi and M. Ichikawa
1571
Role of Oxygen in the SCR of NOx with Propane over Co/ZSM-5: Reaction and TPD Study A. Yu. Stakheev, C. W. Lee, S.J. Park and P.J. Chong
1579
Sharp Contrast in Thermal Stability between MFI-Type Metallosilicates and Metal-Ion-Exchanged ZSM-5 and Their Catalytic Performances for NO Removal S. Iwamoto, S. Kon, S. Yoshida and T. Inui
1587
Formation of Active Sites for Reduction of NO2 with Methane by Solid State Exchange of ln203 into H-Zeolites M. Ogura, N. Aratani and E. Kikuchi
1593
Purification of NOx on Pt-ZSM-5 and Mg-Cu-ZSM-5 Catalysts under LeanBurn Engine Emission Conditions S. Choung, B. Shin and J. Bae
1601
The In-situ Characterization of Titanium Oxides Prepared in the Zeolite Cavities and Framework and Their Photocatalytic Reactivities for the Direct Decomposition of NO into N2 at 275K Y. IchihashL H. Yamashita and M. Anpo
1609
xxiii Photocatalytic Decomposition of Trichloroethylene over Aluminosilicate Zeolites with Isomorphous Incorporation of Titanium I.H. Cho, J.H. Kwak, R. Ryoo, W.S. Ahn, K.Y. Jung and S.B. Park
1617
Catalytic Decomposition of Organic Sulfur Compounds - Effect of Zeolite Acidity M. Ziolek, P. Decyk, J. Czyzniewska and H.G. Karge
1625
Use of Natural Clinoptilolite for the Optimization of Mineral Clay Liners for Waste Deposits M. W. Upmeier and K.A. Czurda
1633
Removal of Highly Concentrated Ammonium Ions by Natural Mordenite S. Noda
1641
Palladium Ion-Exchanged SAPO-5 for a Low Temperature Combustion of CI-h Y. Takita, T. lshihara, H. Nishiguchi and H. Sumi
1647
Kinetics of CH4 Complete Oxidation on CuH-ZSM-5 Catalyst A. V. Kucherov, N. V. Nekrasov, A.A. Slinkin, E.A. Katsman and S.L. Kiperman
1655
Ion-Exchange Behavior of Zeolite NaA and Maximum Aluminum Zeolite NaP E.v.R. Borgstedt, H.S. Sherry and J.P. Slobogin
1659
Zeolite MAP: the New Detergent Zeolite C.J. Adams, A. Araya, S.W. Carr, A.P. Chapple, K.R. Franklin, P. Graham, A.R. Minihan, T.J. Osinga and J.A. Stuart
1667
Part C VI. Adsorption and Diffusion Zeolites as Adsorbents and Catalysts. The Interactive System Encaged Molecule/Zeolite Framework D. Barthomeuf
1677
Methanol Adsorption and Activation by Zeolitic Protons S.R. Blaszkowski and R.A. van Santen
1707
xxiv Carbon Dioxide Adsorption Kinetics in the Presence of Light Paraffins on NaA and CaA Zeolites A. Khodakov and L. V.C. Rees
1715
Specific Adsorption from Aqueous Phase on Apolar Zeolites C. Buttersack, 1. Fornefett, J. Mahrholz and K. Buchholz
1723
Adsorption Studies on Ordered Mesoporous Materials (MCM-41) J. Jdinchen, M. Busio, M. Hintze, H. Stach and J.H.C. van Hooff
1731
Rapid-Scanning FT-IR Study on the Adsorptions of Methanol and Water on H-ZSM-5 Zeolite F. Wakabayashi, M. Kashitani, T. Fujino, J.N. Kondo, K. Domen and C. Hirose
1739
Onthe Sorption of Ethylbenzene in ZSM-5 R. Schumacher, P. Lorenz and H. G. Karge
1747
Ethylene Adsorption on HNaZSM-5: Kinetic Study S.N. Vereshchagin, N.P. Kirik, N.N. Shishkina and A. G. Anshits
1755
Adsorption of Acetylacetone on Layer Silicate Containing Various Interlayer Cations JR. Sohn and S.I. Lee
1763
Sorption of Water Vapor on HZSM-5 Type Zeolites T. Sano, T. Kasuno, K. Takeda, S. Arazaki and Y. Kawakami
1771
~H-NMR Relaxation Times of Water and Benzene Adsorbed in Zeolite Beta S. Sardar, W.D. Basler and H. Lechert
1779
Adsorption of Sulfur Dioxide on Y-Type Zeolites Y. Teraoka, Y. Motoi, H. Yamasaki, A. Yasutake, J. Izumi and S. Kagawa
1787
Vanadium Derivatives of MFI Type Molecular Sieves Investigated by Sorption and Catalytic Tests J. Kornatowski, M. Sychev, M. Rozwadowski and W. Lutz
1795
Desiccant Selection Criteria for Enthalpy Exchange Systems M.P.F. Delmas, W.D. Holeman, C.N. Blystad, W.A. Belding and J.H.D. Tantet
1803
XXV
Atomistic Mechanism of the Adsorption of CFCs in Zeolite as Investigated by Monte Carlo Simulation K. Mizukami, H. Takaba, Y. Oumi, M. Katagiri, M. Kubo, A. Stirling, E. Broclawik, A. Miyamoto, S. KobayashL S. Kushiyama and K. Mizuno
1811
The Crystal Structures of Dehydrated Fully Cd2+-Exchanged Zeolite X and of Its Carbon Monoxide Sorption Complex S.B. Jang, J.H. Kwon, S.H. Song, Y. Kim and K. Serf
1819
Structural Property of Methane(CD4) and Hydrogen(D2) Sorbed Phases on MCM-41 (0=25A) J.P. Coulomb, C. Martin, Y. Grillet, P.L. Llewellyn and J. Andr~
1827
Composition, Location, Modes of Formation and of Removal of Coke Deposited on a 5A Adsorbent P. Magnoux, M. Misk, G. Joly, S. Jullian and M. Guisnet
1835
Self-Diffusion and Diffusive Transport in Zeolite Crystals J. Kdirger and D.M. Ruthven
1843
Simulation of Hydrocarbon Diffusion in Zeolites E.J. Maginn, R.Q. Snurr, A.T. Bell and D.N. Theodorou
1851
Methane Diffusion in Zeolites of Structure Type LTA in Dependence on Physical and Chemical Parameters- An MD Study S. Fritzsche, 3/1. Gaub, R. Haberlandt, G. Hofmann, J. Kgirger and M. Wolfsberg
1859
Study of the Molecular Diffusion in the Internal Porosity of ZSM-5 and HMOR Zeolites L.C. de M~norval, J.G. Kim and F. Figueras
1867
Single File Counterdiffusion in Pores of Infinite and Finite Length J.M..D. MacElroy and S.-H. Suh
1875
Hydrogen Separation by Two-Bed PSA Process J. Yang, J.-H. Lee, C.-H. Lee and H. Lee
1883
Pressure Swing Adsorption of Organic Solvent Vapors on Mesoporous Silica Molecular Sieves S. Namba, N. Sugiyama, M. Yamai, I. Shimamura, S. Aoki and J. lzumi
1891
xxvi
VII. Modifications Post-Synthesis Modification of Microporous Materials by Solid-State Reactions H. G. Karge
1901
A New Layered (Alumino) Silicate and Its Transformation into a FER-Type Material by Calcination L. Schreyeck, P. Caullet, J.C. Mougenel, J.L. Guth and B. Marler
1949
From the Keggin Complex Containing Solution to Pillared Layer Clays - A Comprehensive NMR Study J.B. Nagy, J.-C. Bertrand, L Pdlink6 and L Kiricsi
1957
Inactivation of Acid Sites on External Surface of Zeolites with Methoxytripropylsilane J.-H. Kim, M. Okajima and M. Niwa
1965
Generation of Acid Sites by Incorporation of Cobalt in the AFR Structure J.P. Lourengo, M.F. Ribeiro, F.R. Ribeiro, J. Rocha, Z Gabelica, B. Onida and E. Garrone
1973
Acidic Properties of Galliosilicate Molecular Sieves with the Offretite Structure M.L. Occelli, H. Eckert, C. Hudalla, A. Auroux, P. Ritz and P.S. Iyer
1981
The Thermal Expansion of the Zeolites MFI, AFI, DOH, DDR and MTN in Their Calcined and as Synthesized Forms S.H. Park, R.-W. Grofle Kunstleve, H. Graetsch and H. Gies
1989
Activity Enhancement of H-Zeolites by Ag Ion-Exchange and Sulfiding with Hydrogen Sulfide M. Sugioka and L. Andalaluna
1995
Effect of Pre-dealumination by (NI-h)zSiF6 on the Properties of ZSM-5 with Steam Aging Treatment L. Huang, Q. Li, Z. Xue, G. Ding, G. Niu, Z. Li and Z. Shi
2003
Effect of the Dealumination Procedure on Surface Properties and Catalytic Performance of UHP-Y Zeolite Z. Chang, C. Ruan and G. Tong
2011
xxvii Formation of Alkali Nanoparticles in NaY Zeolite Cages and in A1PO4-5 Molecular Sieves: NMR Studies L. C. de M~norval and F. Rachdi
2019
Iridium in Pentasil: Redox Behavior and Reactivity T. V. Voskoboinikov and E.S. Shpiro
2027
Para-Chlorination Activity of Solid-State Ion-Exchanged Zeolite KL Catalysts J. ~ Yoo, D.S. Kim, J.-S. Chang and S.-E. Park
2035
Solid-State Ion Exchange of Fe(III) into Y Zeolite under Deep-Bed Conditions P. Hudec, A. Smieskovd, Z. Zidek, ~ Jorik, 3/1. Miglierini and J.B. Nagy
2043
Preparation, Characterization, and Catalysis of lntrazeolite Iron Oxide Clusters Y. Okamoto, H. Kikuta, Y. Ohto, S. Nasu and O. Terasaki
2051
Zeolite Pore Size Engineering by Chemical Liquid Deposition Y.-H. Yue, Y. Tang and Z. Gao
2059
Incorporation of Molybdenum into Mesoporous MCM-41 S.D. Djajanti and R.F. Howe
2067
Chemical Vapor Deposition on Basic Zeolites Y. Chun, Q.-H. Xu, A.-Z Yan and X. Ye
2075
Metal-Oxide Interactions and Catalytic Behaviors of La203- and V2OsPromoted Rh/NaY Catalysts K. KunimorL K. Yuzaki, T. Yarimizu, fill.. Seino and S. Ito
2083
VIII. Novel Materials Modification of a Pyroelectric Detector by Controlled Electrocrystallization of Thin Zeolite Layers G.J. Klap, M. Wiibbenhorst, J. van Turnhout, J.C. Jansen and H. van Bekkum
2093
Fabrication, Luminescence and Photoacoustic Spectroscopic Studies of the Semiconductor Nanoclusters in Zeolites G. Tel'biz, 1. Blonskij, S. Shevel and E Voznyi
2101
xxviii Zeolites as Sensitive Materials for Organic Vapour Detection: An Exploratory Study C. CantalinL M. Pelino, M. Pansini and C. Colella
2109
Adsolubilization Equilibrium of Rhodamine B by Zeolite/Surfactant Complexes K. Hayakawa, A. DobashL Y. Miyamoto and L Satake
2115
Investigations into the Engineering of Inorganic/Organic Solids: Hydrothermal Synthesis and Structure Characterization of One- and TwoDimensional Molybdenum Oxide Polymers Y. Xu, L.L. Koh, L.H. An, D.G. Roshan and L.H. Gan
2123
Synthesis and Structure of Cadmium Chalcogenide Beryllogermanate Sodalites S.E. Dann andM.T. Weller
2131
Optical and Magnetic Properties of Na-K Alloy Clusters Incorporated into LTA T. Kodaira, E Nozue, O. Terasaki and H. Takeo
2139
Growth of Oriented Molecular Sieves on Organic Layers S. Feng and T. Bein
2147
Factors Affecting the Porosity of ZSM-5 Layer on the Surface of Stainless Steel Z. Shah, E. Min and H. Yang
2155
Synthesis of Films of Oriented Silicalite-1 Crystals Using Microwave Heating J.H. Koegler, A. Ararat, H. van Bekkum and J. C Jansen
2163
News from AiPO4-5: Microwave Synthesis, Application as Medium to Organize Molecules for Spectroscopy and Nonlinear Optics, Material for One-Dimensional Membranes J. Caro, F. Marlow, K. Hoffmann, C Striebel, J. Kornatowski, 1. Girnus, M. Noack and P. KOlsch
2171
Silylation of Silicalite Membrane and Its Pervaporation Performance T. Sano, K. Yamada, S. Ejiri, M. Hasegawa, Y. Kawakami and H. Yanagishita
2179
Vertically-Aligned MeAPO4-5 Crystals Grown on Anodic Alumina Membrane K.£ Chao, CN. Wu, H.C Shih, T.G. Tsai and Y.H. Chiou
2187
xxix Synthesis ofFER Membrane on an Alumina Support and Its Separation Properties N. Nishiyama, K. Ueyama and M. Matsukata
2195
Synthesis of Ultra Thin Films of Molecular Sieves by the Seed Film Method J. Hedlund, B.J. Schoeman and J. Sterte
2203
Synthesis of SAPO-34/Ceramic Composite Membranes L. Zhang, M. Jia and E. Min
2211
Synthesis of ZSM-5 Zeolite Membrane on the Inner Surface of a Ceramic Tube H.-S. Oh, M.-H. Kim and H.-K. Rhee
2217
Synthesis of Oriented Zeolite Film on Mercury Surface Y. Kiyozumi, F. Mizukami, K. Maeda, T. Kodzasa, M. Toba and S. Niwa
2225
Growth of Oriented Zeolite Crystal Membranes M. Cheng, L. Lin, W. Yang, Y. Yang, Y.-D. Xu and X. Li
2233
Preparation of Fibrous Titanium Silicalite-l(FTS-1) from Nano TS-1 Crystals K.T. Jung, J.H. Lee, J.H. Hyun, D.S. Kim, J. G. Kim and Y.G. Shul
2241
IX. Theory Structure of the Linear Na32÷ Cluster in Zeolite X W. Shibata and K. Serf
2251
Supralattices: Another Dimension in Materials Science- Theoretical Investigation A.A. Demkov and O.F. Sankey
2259
Experimental and Theoretical Studies of Siliceous Zeolites A.K. Cheetham, L.M. Bull and N.J. Henson
2267
Charge-Transfer Molecular Dynamics ofProtonated Faujasite L.J. Alvarez, P.B. Giral, C.Z. Wilson andJ.E. Sdnchez-S6nchez
2275
Quantum-Chemical Study of Hydride Transfer in Catalytic Transformations of Paraffins on Zeolites KB. Kazansky, M. K Frash and R.A. van Santen
2283
XXX
Computer Modelling of the Structure and Synthesis of Microporous and Mesoporous Materials D. l~. Lewis, R.G. Bell, P.A. Wright, C.R.A. Catlow and J.M.. Thomas
2291
Ab Initio Computer Modelling of Zeolite Frameworks I. Modelling of Basic Clusters M. Sato and H. Uehara
2299
Intrinsic and Enhanced Broensted Acidity in Zeolites J. Dwyer, K Zholobenko, A. Khodakov, S. Bates and M.A. Makarova
2307
Molecular Sieve Effect of Chemically Modified Na-A Type Zeolite and Its Molecular Dynamic Simulation J. lzumi, A. Yasutake, N. Tomonaga, N. Oka, H. Ota, N. Akutsu, S. Umeda andlVl. Tafima
2315
Computational Study of Structural and Thermal Properties of the Microporous Titanosilicate ETS- 10 M.E. Grillo, J. Lujano and J. Carrazza
2323
Complete Redox Exchange of Indium for TI÷ in Zeolite A. Synthesis and Crystal Structure of Fully Indium-Exchanged Zeolite A N.H. Heo, H.C. Choi and K. Serf
2331
Location and Orientation of Pyrrole and Acetaldehyde Molecules inside Siliceous Faujasite as Predicted by Electronic Structure Calculations A. Chatterjee, R. Vetrivel, M. Kubo and A. Miyamoto
2339
Commensurate Freezing of Hydrocarbons in Silicalite IJ(.jM. van Well, J.P. Wolthuizen, B. Stair, J.H.C. van Hooff and R.A. van Santen
2347
Phase Transition Types Observed During the Sorption of van der Waals Gases on Model Zeolites: Silicalite I and AIPO4-5 J.P. Coulomb, C. Martin, P.L. Llewellyn and Y. Grillet
2355
Author Index
2363
Subject Index
2375
xxxi
Preface The 11th International Zeolite Conference was held successfully in Seoul, Korea, from August 12 to 17, 1996. The main conference was preceded by the Pre-Conferenee Summer School on Zeolite held in Taeduck Science Town and followed by the PostConference Symposium on Catalysis related to Environmental Application of Zeolite in Kyoungju, Korea. We would like to thank members of the IZA Council, liaison to the council, Dr. Ono, and members of the International Advisory Board for their active support for the conference. The number of registrants totaling about 500 was a little bit less than the organizing committee hoped for. Considering the shortened interval between the successive International Zeolite Conference from three to two years, this number nevertheless reflected quite a favorable response to this conference. During the 6 day meeting of the main conference 5 plenary lectures and 113 papers were presented orally in 40 sessions and 165 full papers as well as 127 recent research reports were presented as posters. Ever increasing interest and continuous developments in the zeolite science and technology are reflected in the number of submitted contributions in various areas of research and application. We would like to thank all those who have submitted the papers. It is regrettable, however, we could not accommodate many contributions of high quality due to the limited time and space available for presentation. We also had to make certain consideration on the balance among the different disciplines. Each manuscript for the proceedings was reviewed by two reviewers and in case of a conflicting reviewing results a third referee was asked to recommend as to the acceptance of the paper for publication in the proceedings. The organizing committee is most grateful to the experts who spared their precious time to review abstracts as well as the full manuscript for the proceedings. Our special appreciation goes to Dr. David Olson who headed the third referee group. The Proceeding of the 1l th Zeolite Conference is published in three volumes containing 5 plenary lectures and 274 full papers. Part A contains Synthesis and Characterization (99 papers), Part B Catalysis, Environment (102 papers), and Part C Adsorption and Diffusion, Modifications, Novel Materials and Theory (78 papers).
xxxii Although 161 papers out of 279 are presented as posters no difference is made whatsoever between the oral and poster papers in publishing the full manuscript in the proceedings. Zeolite catalysis has been and continues to be an area of major interest. Growing interest in the synthesis, and the characterization of zeolite and microporous materials is reflected in the large number of contributions. Other area of growing interest is novel materials. Adsorption, theory and modeling remain as attractive areas. Our ambitious original plan to publish the proceedings before the conference had to be modified and three volume proceedings will be published by the end of this year. Generous donations were received from a number of organizations whose names are given in the sponsor's list. The organizing committee is most grateful to them for their support. Finally we would like to express our sincere appreciation to the authors for their fine papers and all the reviewers who made careful reviewing of the submitted abstracts. We are also grateful to the members of the scientific committee who have spent so much time and effort to select the papers, especially to Prof. Gon Seo, Prof. Yang Kim, Prof. Jong Rack Sohn, Dr. Sang-Eon Park, and Prof. Ryong Ryoo. We would like to thank also Mr. Sang lck Lee and Dae-Chul Kim who helped in the preparations of the proceedings.
Seoul, August, 1996
Hakze Chon Son-Ki Ihm Young Sun Uh
xxxiii
Organizing Committee of the 1 lth IZC Chairman Hakze Chon
Korea Advanced Institute of Science & Technology, Taejon, Korea
Vice-Chairmen Hanju Lee Baik-Hyon Ha Wha Young Lee
Yonsei University, Seoul, Korea Hanyang University, Seoul, Korea Seoul National University, Seoul, Korea
Secretary Young Sun Uh
Korea Institute of Science & Technology, Seoul, Korea
Finance Sub-Committee Chairman Hanju Lee
Yonsei University, Seoul, Korea
Members Hyun-Ku Rhee Ki Woong Sung Bong H. Chang
Seoul National University, Seoul, Korea. DaeLim Industrial Co., Ltd., Seoul, Korea AeKyung-PQ Advanced Materials Co. Ltd., Seoul, Korea
Program Sub-Committee Chairman Sang Heup Moon Members Wha Seung Ahn Suk-Jin Choung Sung Hwan Han Suk In Hong Kyung Lim Kim Ho-ln Lee
Seoul National University, Seoul, Korea
Inha University, Inchon, Korea Kyunghee University, Suwon, Korea Korea Institute of Science & Technology, Seoul, Korea Korea University, Seoul, Korea Yonsei University, Seoul, Korea Seoul National University, Seoul, Korea
xxxiv Hyun Ryul Park Tae-Jin Park Kee Jun Yoon
Chungang University, Seoul, Korea Korea Institute of Science & Technology, Seoul, Korea Sungkyunkwan University, Suwon, Korea
Scientific Sub-Committee Chairman Son-Ki lhm
Korea Advanced Institute of Science & Technology, Taejon, Korea
Vice-Chairman Gon Seo Members Byung Joon Ahn Hee Kwon Chae Paul J. Chong Jong Shik Chung Kee Sung Ha Chong Soo Han Nam Ho Heo Suk Bong Hong Seon-Yong Jeong Wha Joong Kim Jae Chang Kim Man Hoe Kim Yang Kim Chul Wee Lee Dong-Keun Lee Jae Sung Lee Jung-Min Lee Tae Jin Lee Hee Moon Sang Sung Nahm In-Sik Nam Kyung Tae No
Chonnam National University, Kwangju, Korea
Chonbuk National University, Chonju, Korea Hankuk University of Foreign Studies, Yong-ln Korea Korea Research Institute of Chemical Technology, Taejon, Korea Pohang University of Science and Technology, Pohang, Korea Pusan National University of Technology, Pusan, Korea Chonnam National University Kyungpook National University Korea Institute of Science & Technology, Seoul, Korea Korea Research Institute of Chemical Technology, Taejon, Korea Konkuk University, Seoul, Korea Kyungpook National University, Taeku, Korea Air Force Academy, Chongju, Korea Pusan National University, Pusan, Korea Korea Research Institute of Chemical Technology, Taejon, Korea Kyeongsang National University, Taeku, Korea Pohang University of Science and Technology, Pohang, Korea Korea Research Institute of Chemical Technology, Taejon, Korea Yeungnam University, Taeku, Korea Chonnam National University, Kwanju, Korea Korea Research Institute of Chemical Technology, Taejon, Korea Pohang University of Science and Technology, Pohang, Korea Soongsil University, Seoul, Korea
XXXV
Korea Advanced Institute of Science & Technology. Taejon, Korea Seung Bin Park Korea Research Institute of Chemical Technology, Taejon, Korea Sang-Eon Park Korea Advanced Institute of Science & Technology, Taejon, Korea Ryong Ryoo Yonsei University, Seoul, Korea Yong Gun Shul Kyungpook National University, Taeku, Korea Jong Rack Sohn Korea Institute of Science & Technology, Seoul, Korea Dong-Jin Suh Hongik University, Seoul, Korea Sung-Sup Suh Korea Advanced Institute of Science & Technology, Taejon, Korea Seung lhl Woo Ajou University, Suwon, Korea Jae Eui Yie Kyung Byung Yoon Sogang University, Taejon, Korea Jong-Sung Yu Hannam University, Taejon, Korea
Pre-Conference Summer School on Zeolites Chairman
Seung lhl Woo
Korea Advanced Institute of Science & Technology, Taejon, Korea
Co-Chairman
Sang-Eon Park
Korea Research Institute of Chemical Technology, Taejon, Korea
Members
Byung Joon Ahn Oh Bong Yang Sang Sun Nahm
Chonbuk University, Chonju, Korea Chonbuk University, Chonju, Korea Korea Research Institute of Chemical Technology, Taejon, Korea
Post-Conference Symposium on Catalysis Chairman
Young Gul Kim
Pohang University of Science and Technology, Pohang, Korea
Member
In-Sik Nam Kyung Hee Lee Jong Shik Chung Jae Sung Lee
Pohang University of Science and Technology, Pohang, Korea Pohang University of Science and Technology, Pohang, Korea Pohang University of Science and Technology, Pohang, Korea Pohang University of Science and Technology, Pohang, Korea
xxxvi
International Advisory Board A. Alberti J.R. Anderson J.N. Armor R. von Ballmoos
T. Bein A.T. Bell H. van Bekkum G. Bellussi H.K. Beyer D.M. Bibby M. Btilow K.-J. Chao A. Corma E.G. Derouane J. Dwyer F. Fajula
F. Fetting E.M. Flanigen P. Gallezot D. Goldfarb L. Guczi X. Guo A.B. Halgeri W. H01derich J. van Hooff R.F. Howe T. Inui K. lone P.A. Jacobs K.-J. Jens
S. Kaliaguine
University of Ferrara, Italy Monash University, Victoria, Australia Air Products & Chemicals Inc., USA Engelhard Corp., Ohio, USA Purdue University, Ind, USA University of California, Berkeley, USA Delft University of Technology, The Netherlands Eniricerche, Milano, Italy Hungarian Academy t?fSciences, Hungary The New Zealand Inst. For Ind. Res. & Dev., New Zealand The BOC Group Technical Center, USA National Tsing Hua University, Hsinchu, Taiwan Valencia University of Technology, Spain University of Namur, Belgium University of Manchester, UK ENSCM, Montpellier, France Darmstadt University of Tech., Germany UOP, Tarrytown, USA Institut de Recherches sur la Catalyse, France Weizmann Institute of Science, Israel Hungarian Academy of Sciences, Hungary Chinese Academy of Sciences, China Indian Petrochemicals Corp., India RWTH Aachen, University of Tech., Germany Eindhoven University of Tech., The Netherlands University of New South Wales, Australia Kyoto University Kyoto, Japan Boreskov Inst. of Catalysis, Novosibirsk, Russia Katholieke Universiteit, Leuven, Belgium Statoil Petrochemicals and Plastics, Norway Universit~ Laval, Canada
xxxvii
J. Kiirger
Hungarian Academy of Sciences, Hungary Fritz Haber Institute, Max Planck Society, Germany University of Leipzig, Germany
V. Kaub,i~,
University of Ljubljana, Slovenia
H. Kessler
University of Haute Alsace, France Ryukoku University, Japan Woodbury, NJ, USA Helsinki University of Technology, Finland University of Twente, The Netherlands University of Kiel, Germany Worcester Polytech. Inst., USA Katholieke Universiteit Leuven, Belgium ETH-Zentrum, Ziirich, Switzerland ETH-Zentrum, Zi~rich, Switzerland Res. Inst. of Petroleum Processing, China The Nishi-Tokyo University, Japan CNRS, Villeurbanne, France Biosym Technologies Inc., USA University of Cape Town, South Africa Mobil R&D Corp., USA Tokyo Inst. of Tech., Japan University of Leipzig, Germany National Chemical Lab., Pune, India University of Edinburgh, UK University of Maine, USA Northwestern University, Ill., USA Eindhoven University of Tech., The Netherlands Gunma University, Japan Sophia University, Japan Russian Academy of Sciences, Russia University of California, Santa Barbara, USA University of Connecticut, Conn., USA University of Clark Atlanta, Ga., USA University of Tokyo, Japan
D. Kall6 H.G. Karge
M. Koizumi G.T. Kokotailo A.O.I. Krause J.A. Lercher F. Liebau
E. Ma J. Martens L.B. McCusker W.M. Meier E. Min S. Namba C. Naccache J.M. Newsam C.T. O'Connor D.H. Olson Y. Ono H. Pfeifer P. Ratnasamy L.V.C. Rees D.M. Ruthven W.M.H. Sachtler R.A. van Santen
M. Sato K. Segawa E.S. Shpiro G.D. Stucky
S.L. Suib R. Szostak T. Tatsumi
xxxviii J.M. Thomas R.P. Townsend J.W. Ward J. Weitkamp T.E. Whyte, Jr T. Yashima R. Xu K.I. Zamaraev M. Zi61ek
The Royal Institution of Great Britain, UK Unilever Research, Bebington, UK UOP, Brea, USA University of Stuttgart, Germany The PQ Corporation, Conshohocken, USA Tokyo Inst. of Tech., Tokyo, Japan Jilin University, Changchun, China Boreskov Inst. of Catalysis, Novosibirsk, Russia Adam Mickiewicz University, Poznan, Poland
Liaison to the 11 th IZC Y. Ono
Tokyo Institute of Technology, Tokyo, Japan
Members of the IZA Council Roland von Ballmoos
President
Jens Weitkamp
Vice President
Koos Jansen
Secretary
J. Michael Bennett
Treasurer
T. Bein, G. Bellusi, K.-J. Chao, H. Chon, T. Inui, H. Karge, L.B. McCusker, W.J. Mortier, D.E.W. Vaughan, T. Yashima, S.I. Zones
xxxix
Financial Support The Organizing Committee gratefully acknowledges support by the following institutions and companies: (As of August 30, 1996) Korea Science and Engineering Foundation, Seoul, Korea Korea Research Foundation, Taejeon, Korea LG-Caltex Oil Corporation, Seoul, Korea YukongLimited, Seoul, Korea SsangYong Oil Refining Co., Ltd., Seoul, Korea DaeLim Industrial Co., Ltd., Seoul, Korea AeKyung-PQ Advanced Material Co., Ltd., Seoul, Korea Samsung Fine Chemicals Co., Ltd., Seoul, Korea Korea General Chemical Corporation, Seoul, Korea Zeobuilder Co., Ltd., Seoul, Korea Isu Chemical Co., Ltd., Seoul, Korea Cosmo Industrial Co., Ltd., Cheong-ju, Korea
This Page Intentionally Left Blank
I.
Synthesis
This Page Intentionally Left Blank
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 1997 Elsevier Science B.V.
DIRECTED SYNTHESIS OF ORGANIC/INORGANIC COMPOSITE STRUCTURES
Galen D. Stucky, Qisheng Huo, Ali Firouzi, and Brad F. Chmelka Departments of Chemistry, Materials, and Chemical Engineering University of California, Santa Barbara, CA 93106, U.S.A.
Stefan Schacht, I. G. Voigt-Martin, and Ferdi Sehiith Institut ftir Anorganische Chemie, Frankfurt University, Frankfurt, Germany
1. INTRODUCTION The impact of the discovery of the synthesis of periodic mesoporous material using amphiphilic surfactants 1,2,3,4,5,6 is readily apparent from the demographics of papers that have appeared in this area, as illustrated in Figure 1 for MCM-41 publications. In addition to providing for the first time access to high surface area, monodispersed mesopores (lnm to > 10nm), the research has provided, in a more generic sense, a new synthesis paradigm on how to bring together spatially distinct, nanostructured organic and inorganic arrays into two- and threedimensional periodic, composite structures. Designed materials synthesis and properties based on the molecular level interplay of the kinetics and energetics of organic and inorganic domain and interface
200-,,,,
assembly are of vital interest to many areas including biomineralization, conducting and optical display polymer composites, chemical sensors, fine chemical and bio-catalysis, and the creation of composite phases with useful
mechanical
and
.o 150 .~ "~ ~ 100 "~, 50
....................
J
i
................
~ .................
~ .................
~ .................
................
~ .................
~.................
~ .....................................................
thermal
properties for insulation and packaging applications. It is clear that this discovery is a major entry not only in the "breakthrough" library of zeolite and molecular sieve syntheses, but also
o
....
1991
*
....
....
i
~
................
~................
. . . . . . . . . . .
,
1 9 9 2 1993 1 9 9 4 1995 1 9 9 6 1997 Year
Figure 1 MCM-41 publications as found by STN of the American Chemical Society. The value for 1996 is an extrapolation based on the first five months.
in advancing the field of materials synthesis in general. In this paper, I will focus on some observations concerning this composite synthesis paradigm. The presentation is admittedly only a very selected sampling, with some brief excursions into implications related to biomineralization and porous materials design at longer (10 nm to 1000nm) length scales. Much progress has been made 7,8,9,10,11,12,13,1't,15,16 in what has been appropriately described as the "lofty goal of molecular sieve synthesis by design ''17. For these microporous (<15/~) phases, organic-inorganic (OI) interactions dominate during synthesis while what is generally the kinetically slower inorganic condensation (II) progresses so that each structure directing agent (SDA) is encapsulated within a cage and/or pore opening with only secondary van der Waals organic-organic (OO) interactions found in the final product (Figure 2, OI > OO, II > OO).
Charge matching of the available charge/unit area of the organic with that of the I Inorganic Molecular Species ~
HO
+ n[~
~
~}
~
~ O ~ Organic ' ~ - ~ Molecules/Arrays X"
Interface .S~ssembly
N ~N
Ol > OO
-
O > Ol II "Biomimetics" ' ~ . . ~
/
%~-~o
.. ~ SEQUENr~L
FLMGROWTH
OO,II << OI
/
II > OO
~ ~'. ~~'
Organic/l~t~organic Array A.,sembly ~,~,~ ~ q~
Inorganic Polymerization On OrganicArrays MESOPOROtSTmN FILMS
/
/
EMULSION"TEMPLArING~' Silica Acid Synthesis
MOLECULAR SIEVES
~
~.MESOPOROI.S MATERIALS
//~v
Silica Base Synthesis
Inorganic Polymerization Figure 2 Schematic illustrating organic-organic (OO), organic-inorganic (OI) interface, and inorganic-inorganic (II) control of composite materials synthesis. The ordering processes kinetically and/or thermodynamically determined and also must include solvation and cosolvent effects
encapsulating inorganic is required. Water molecules of solvation play a key role in this assembly process, both in terms of solubilizing the SDA and as an entropic thermodynamic driving force provided upon release of the water molecules as inorganic-organic assembly takes place. Taking into account these various factors, rigid, bulky and relatively short (<10A for the longest axis) molecules with moderate hydrophobicity are the best SDAs for high-silica molecular sieve synthesis 17. If solvation and cosolvent effects are for the moment implicitly included in the OO, OI, and II assembly processes, an interesting variation in materials synthesis takes place if OO, II are both much less kinetically and/or thermodynamically favorable than OI (OO, II << OI in Figure 2). This permits the very clever sequential growth process developed by Mallouk 18,19, in which monolayers of organic, then inorganic, etc., composition can be deposited to give lamellar phases that can be structurally designed over more than 100 repeats. This spatial control of composite ordering makes it possible to alter, for example, every nth repeating unit or to create compositionally laddered Ionic
arrays. The two situations of particular interest in this discussion arise when OI > OO>Ilor
O O > O I , II.
Again
should
it
emphasized
that
be these
Covalent
I / o-
I
o-
~
Silicate Anion Oligomer
ordering processes can be Bilayer (Base Synthesis) kinetically thermodynamic determined.
and/or ally
,o,o. 0
0 \ O" NSi/ Si" O/ ~ O / \ O \ H
Direct Framework Surfactant Inclusion Figure 3 Strong ionic 1-6 and covalent 20-22 interface bonding in silica mesostructure assembly.
The first situation with OI > OO; OO,II << OI (Figure 3) suggests that one can expect the original organic array, if present, to be disrupted upon interaction with the inorganic species; and then to reorganize to a new configuration determined by kinetic and thermodynamic assembly parameters associated with the newly formed molecular or oligomeric organic-inorganic unit. The formation constant for OI is large in this case with strong OI bonding due to interactions such as multidentate binding and chelation, or the forces between highly charged inorganic/organic species. The same result is obtained by creating the organic-inorganic molecular or oligomeric unit using covalent bonding20,21, 22 (Figure 3) between the desired organic and inorganic moieties. This
situation has been recently experimentally confirmed by in situ studies of the base (pH > 9) synthesis of mesoporous silicate phases using colloidal silica and cetyltrimethylammonium cations as the surfactant amphiphile23,24; and by the use of covalently bound organosilicon or transition metal 25 organometallic precursors in mesoporous phase synthesis. The second situation (OO > OI, II Figure 2) means that an organized organic array controls the assembly and also defines the ultimate configuration of the composite phase. In fact, this is the basis for what has been described as a central tenet of biomineralization 26,27,28,29,30,31that states that nucleation, growth, and the final morphology of biominerals are determined by the existence of a preorganized assembly of organic molecules. "Biomimetic" approaches and modelling of biomineralization have relied on this paradigm for experimental design and have accordingly focused on the use of known stable organic arrays or stabilization through, for example, covalent attachment to a substrate or crosslinking of the organic groups. Some examples include (i) hollow submicro-diameter silica cylinders obtained by depositing silica onto phospholipid tubules 32, (ii) bulk inorganic iron oxide deposited on charged bio-lipid substrates 33, and (iii) ceramic thin film processing by deposition of bulk inorganic phases on surfaces functionalized with ionic organic surfactants 34. A well known biological example of a strongly bound organic array whose surface is used as a template for inorganic oxide aggregation is apoferritin. Since composite assembly is determined by the
Hydrogen Bonding
relative strengths of the thermodynamic driving forces and the relative rates of the kinetic processes, stabilized organic arrays do not have be used if the OI binding interaction is weak. An example is the tri-layer (S§
35 hydrogen
bonding shown in Figure 4 that is obtained by combining cationic surfactants with cationic silica species at acidic pH values below the aqueous silica isoelectric point (SIp)36,37. In those cases where one wishes to retain or only slightly
N
N
R/+/~R
R/I~+~
CI" I
CI-
CI- CIi
I
I
modify the organic morphology that exists in the absence of
silica S+ X - I + trilayer (Acid Synthesis)
the silica, the (S§ but not the (S§ 3 base synthesis structure directing approach has been demonstrated to be successful. Examples include the synthesis of mesoporous
Figure 4 Structure direction by hydrogen bonding36,37 in mesostructure synthesis.
thin films on inorganic substrates 38 and at the air-water interface 39, mesostructure templating using
preformed organic liquid crystals 4~ and in the creation of micron scale shaped mesoporous structures by using amphiphilic surfactants embedded in the oil phase of oil-water microemulsions or oil water interfaces (see below).
2. SURFACTANT CONSIDERATIONS It is important to emphasize that the two situations described above (OI > OO > II, and OO > OI, II) are two different synthetic strategies, that not unexpectedly lead to composite and porous materials that have distinctly different properties. These are further described later in this paper. The common denominator for both routes is the dominating role that the surfactants have in determining the overall structural symmetry of the final product, a role also reflected in the observation that the same relatively small group of space group symmetries are obtained for conventional amphiphilic, hydrophilic, and polymer-based surfactant systems even though the underlying compositions, molecular structures, chemical and physical properties differ substantially 4i,42. Among the structures41,43 that can be observed in surfactant or lipid containing lyotropic systems, hexagonal (2d, p6m) and lamellar phases are the two most common mesophases. Six lyotropic cubic phases, in which Pm3n and Ia3d are two typical mesophases, may be found in many surfactant and lipid systems (for a recent review, see reference 42). Several intermediate phases can be formed44,45. Similar systems follow the same succession of phases, but not all of the phases are always present. However, the formations of additional new lyotropic mesophases are also possible, as indicated by the fact that new cubic phases, which consist of micelles of type I (oil-in-water), appear to be present in some surfactant systems46,47,48, 49. However, at this time no clear conclusions about the exact nature of the new phases have been obtained since the quality of the diffraction data is not adequate to determine their structures. Inorganic mesophases with good long-range ordering quality and excellent stability are helpful in characterizing new liquid crystal-like structures. In the conventional charged surfactant-water mixture at a given composition and temperature, from a molecular point of view the micellar shape or packing of the surfactant is determined by a balance between three general types of free energy contributions. One is associated with the tendency of the alkyl chains to minimize their water contact and maximize their inter-organic interactions. The second involves the coulombic and dipolar interactions among the charged headgroups and their associated anions. This contribution determines the mean area-perhead-group, a 0, that is available to each surfactant head group in an aggregate. In most classical discussions of liquid crystal aggregates, the counter-ion of the surfactant is implicitly included in
a o. The third type of free energy contribution includes solvation energies that arise from the presence of water, alcohol, or organic molecules in the hydrophilic, intermediary hydrophobichydrophilic
"palisade",
and
hydrophobic regions. Because
the
synthesis
intermediates and final composite structure are a consequence of the organization of spatially distinct organic and inorganic nanophase regions, the structure can also be readily defined in terms of surfaces generated by the above collective interactions (Figure 5). The mathematical perspective of the structure becomes one based on a differential calculus description of the spatial continuum described by the
Figure 5 Cartoon illustrating hypothetical cross section of mean surface continuums defined by collective interactions of organic surfactants and inorganic species. Curvature is defined by incompatible local packing requirements and structure frustration. The resulting modulated structures may exist in "lamellar", "hexagonal", etc., structured phases.
surfaces rather than the usual matrix algebra that is commonly used to describe a structure consisting of a collection of atoms located at discrete points in spaceSO,51. In this description, the inorganic and organic arrays of these mesostructures meet at an interface surface. The interface curvature is energetically defined so as to optimize charge repulsion and van der Waals interactions, resulting in a minimal surface structure for MCM-48 52,53,54. Phase transitions are associated with changes in the curvature of interface and may be understood phenomenologically as a competition between the elastic energy of bending the interfaces and energies resulting from the constraints of interfacial and charge separation 55. The different entropic and interaction energies in the nanoscale organic, inorganic and interface regions result in structure frustration with incompatible local packing constraints that forbid an optimal geometry where the energy is everywhere minimized. The inorganic/organic structures therefore readily undergo structural changes or transformations 56 to relieve this stress through rotational displacements of the surfaces (disclination defect). This structural modification is experimentally driven by entropic changes in the organic array (temperature), silica polymerization which modifies local density and interface charge properties23,24, 52 or through coordinated solvent (water) and organic cosolvent displacement21,23,24,73.
Because the mesostructured composite phases are frustrated structures, it is not surprising that one finds phases that for example would be classified as lamellar from the standpoint of the relatively crude average structure given by low-angle X-ray diffraction, but in fact on closer inspection by electron microscopy are found to have in-plane modulation, and a periodic rippled lamellar structure 24. BET (Brunaer-Emmett-Teller) measurements of this calcined "lamellar" phase show a high surface area and monodispersed pores. Similarly, there is considerable evidence to expect 3,4,5,56,57 that the honeycomb p6m (MCM-41) structure defined by X-rays very likely includes structures with modulated pores such as those indicated in Figure 5. The implication is that it should be possible to kinetically tune not only pore dimensions3,4,5, 21,37,58 for structures such as MCM-41, but also wall and pore morphologies. The characterization of these modulated structures with periodic necking of the honeycomb pores in a structure like MCM41 requires careful TEM and organic guest absorption/desorption isotherm studies. It is particularly important to note that the symmetries determined by the Bragg peak positions of X-ray or even electron diffraction are best viewed as "average" symmetries and a careful analysis of the diffraction intensities, freeze fracture or cryomicroscopy, solid state NMR, and adsorption or desorption data are required in order to characterize the details of the cage, wall and pore structures. Because of the limited amount of scattering data available for materials with high void densities and large unit cells, diffraction modelling must be done on the continuum surface basis and not at the discrete atom level used for zeolite structure determination. The continuum surface model has been particularly useful in understanding structures and phase transformations of materials in which surfactants play a dominating role in determining the overall structural symmetry, and there is every reason to believe that it applies equally well to inorganic mesostructured composites. However, the chemist begins with precursors defined on a molecular basis so a key question is how to relate these surfaces to surfactant molecular structure. Fortunately several investigators have shown that it is possible to mathematically relate molecular size, charge, and shape to the more global surface curvature, bending energies and morphology5~
The classical and contemporary molecular description of surfactant organization
in amphiphilic liquid crystal arrays has been described in terms of the local effective surfactant packing parameter 59,60, g __ V/a J, where V is the total volume of the surfactant chains plus any co-solvent organic molecules between the chains, a o is the effective head group area at the micelle surface defined above, and 1 is the kinetic surfactant tail length or the curvature elastic-energy55. The interface surface bending energy can be written in terms of g, the actual surfactant packing
10 parameter adopted by the aggregating chains in the phase 5~
The counterion in this classical
model is not explicitly included. It is not immediately clear that this relatively simple molecular model can be used as a first approximation to explain and predict product structure and phase transitions for the inorganic mesostructures.
Our preliminary goal was a very pragmatic one, to determine whether the
molecular packing parameter model used in liquid crystal chemistry is useful in designing inorganic/organic composite mesostructures. In classical micelle chemistry, as the g value is increased above critical values, mesophase transitions occur. The expected mesophase sequence as a function of the packing parameter is : 43,50 Packing Parameter, g Mesophase Example These
1/3
1/2
1/2- 2/3
1
Cubic (Pm3n)
Hexagonal (p6m)
Cubic (Ia3d)
Lamellar
transitions
reflect
a g =
decrease in surface curvature from cubic (Pm3n)
through
lamellar.
For
V/a o i
i,,'j MCM-4 (Pm3n) ,!(P63/mmci!j (p6m) li ;:~
surfactants to associate in a spherical structure, the surface area occupied by the surfactants polar head group should be large.
~i(la3d) i~ i~ sBA-5 ~ SBA-4
!i (R3c)i-!
_~~
If the head groups are
base ~'cltalyzed ~ ' ~
permitted to pack tightly, on the other
I I
I
EinSteinbehavior| Cluster-like I i~ I
hand, the aggregation number will
r..-
Im3m? ti Vj SBA-1 ~SBA-7 i~ SBA-3 (Pm3n) ~(P63/mmc)~,.,~ (pSm~
increase, and rod or lamellar packing will be favored. The values of g (between 1/2 and 2/3) for cubic (Ia3d) phase
~,~
depend upon the volume fraction of surfactant chains 50.
I
For the systematic investigation of
the
formation
~
~ ~ i~
. ;Lamellarl L,i I
~
~,~
acid ~.* -------~ catalyzed i'i
~Li Su "~ be vi r
of mesoporous
materials, we selected a series of surfactants (Figures 7, 8), with and without organic additives, which favor a
Figure 6 Mesophase structures obtained by systematically varying V, ao and 1 of packing parameter.
11
Figure 7. Examples of surfactants used in this research III
IIII
I IIIII
Name
I
Structure Example
ALKYLAMMONIUM CnNR1R2R3 = CnH2n+ 1NR1R2R3 n = 10, 12-16, 19, 20, 22 R = H, Car~2m+ 1
cn3 cH3
m = 1, 2, 3
GEMINIAMMONIUM Cm-s-m CmH2m+IN(CH 3)2(CI-I2)sN(CH3)2CmH2m+I m - 12, 14, 16, 18, 20, 22 s - 2 -12
~
N+
| ~CH3 CH3
DIVALENTS URFACTANT
Cn-s-I CnH2n+1N(CH3)2(CH2)sN(CH3)3 n= 12, 13, 16, 18,20,22 s=2, 3, 6
~H3+
CH3 l+
. N . ~ , , ~ N ~ CH
HYDROXY- FUNCTIONALAMMONIUM CnH2n+IN(CH 3)m[(CH2)POH]3_m n = 16 m = O , 1,2,3 p = 0 , 1,2,3
[§ N~OH
~H3
CH3
BENZALKONIUM
CnH2n+1N(CH3)2(CH2)mC6H5 n = 14, 16, 18,20
m = 1,2,3
BI-CHAIN AMMONIUM CnH2n+ 1N(CH3)2CmH2m+I n = 12, 16, 18 m
cH3 = 2-6,
12, 16, 18
~
\cH3
cH3
~cH3
CnH2n+1[N(CH3)2]m(CI-I2)pSi(OCH3)3
l+
~i__OCH3
n = 14, 18
~H3
ORGANOSILANE
m=0, 1
p=0, 3
cn3
ZWlTrI~RIQN
CnH2n+IN+(CH3)2RXn = 12 - 20 RX-= sulfonate, carbonate,
OCH3
etc
~H~ (Crb.)3-SO3-
12 range of g values when used as structure directing agents to synthesize silica-based mesophases in different reaction conditions. An examination of a large number of surfactants synthesized in our laboratory, some of which are shown in Figure 8, coupled with a study of the effects of cosolvents, has confirmed that to a first and relatively good approximation the molecular packing parameter model can be used in a predictive way to generate structures analogous to those found in conventional liquid crystal chemistry (Figure 6) 36,37,21. For example, if one wishes to create a silica structure in which there is considerable wall curvature and possible
cage
structure,
R1
the
effective head group area can be
R2
R3
Product
R1
H CH 3 CH 3 SBA-3 (p6m) CH 3 CH 3 CH 3 SBA-3 (p6m) CH 3 CH 3 CiH 5 SBA-3 (p6m) I CH 3 CiH 5 CiH 5 SBA- 1 (Pm3n) R3 CiH 5 CiH 5 CiH 5 SBA-1 (Pm3n) Figure 8 Headgroup (ao) definition of mesostructure phase at pH values below the isoelectric point
modified by simple head group I_1. substitution (Figure 8) or with the C16H33 - - N ~ R 2 Cn_s_l surfactants (Figure 7). Cn_s_l surfactants
have
charge
and
density
high large
headgroups, and therefore favor globular micellar aggregates 47. Thus, in an acid media p6m hexagonal phase with symmetry Pm3n are obtained with methyldiethyl or triethyl substitution of the head group (Figure 8), but p6m structures result if dimethyl substitution is used with hydrogen, methyl or ethyl in the third position21,36, 37. Larger surfactants are required in basic media62, and have given unit cells as large as 180/~ on edge, with cell volumes of over 5.8 million/~3. BET data and preliminary modelling of the X-ray diffraction data of the silicate phase 63 suggest a cage structure for Pm3n, similar to those proposed for a conventional liquid crystal Pm3n phase by Sadoc 64 and for the much smaller
Figure 9 Proposed Pm3n structurc for mesosilicate (SBA- 1)
(13.4/~) high temperature unit cell of melanophlogite 65 (Figure 9). A second more subtle and variable way to fine tune the surfactant molecular shape and charge is by using multicharged oligomeric units. This has been done in our laboratory with bi(gemini), tri, tetra and polymeric cationic systems with considerable success. In this discussion,
13 we will briefly review the gemini and divalent surfactants (Figure 7). "Gemini surfactant", Cm.s_m, is a name assigned to a family of synthetic amphiphiles possessing, in sequence, a long hydrophobic chain, an ionic group, a spacer, a second ionic group, and another hydrophobic tail 66,67,68,69. The divalent quaternary ammonium surfactant, Cn_s_ l, may be considered as a end member of gemini surfactant or a highly charged large headgroup surfactant. These surfactants are particularly interesting from a fundamental point of view: their structure can be considerably modified by acting independently on the length and nature of either side chain and the spacer group. The relative positions and distances of headgroups of conventional mono(quaternary ammonium) surfactants are determined primarily by electrostatic interactions and also by the packing requirements of disordered alkyl chains. Formally, the Cm_s_m surfactants
may
be
considered
as
dimers
(double-headed)
of
the
two-chain
CmHEm+I(CHE)s/EN+(CH3)2 surfactants. For bis(dimethylalkyl-ammonium) surfactants, two quaternary ammonium head group species CmHEm+IN+(CH3)2 are chemically linked through an adjustable polymethylene spacer (CsHEs). The presence of the spacer makes it possible to fine tune the distance between the head groups and thereby control the effective head group size, a o , as a function of charge (for detail see reference 70). By this means we can change V/aol of a surfactant by adjusting its spacer length 69. We used the surfactants in this family as structure directing agents in order to synthesize a variety of silica-based mesophase products. Their structure directing behavior is similar to that in surfactant-water binary system 68,69,70,71 and give the structures expected for charge density matching. Small s (2 or 3) surfactants favor MCM-50, medium s (5 or 6) surfactants favor MCM41. C16.12_16 gives MCM-48 at both room temperature and high temperature (100~
while C12 -
12-12gives MCM-41 at room temperature. The latter observation illustrates the ability to fine tune with the individual tail lengths. Note that aqueous solutions of C 12-12-12 remain micellar over the entire range of composition and do not form lyotropic liquid crystal phases 68. This circumstance demonstrates the importance of the inorganic species in the cooperative structure directing mechanism for the concentration region in which the syntheses are carded out. If the tail of one of the two surfactant head groups is eliminated to give a Cn_s_ 1 molecular shape, the effective head group area relative to total hydrophobic tail volume (V) and length (1) is effectively doubled, greatly decreasing g, the packing parameter. This puts us back in the cage
14 side of the structural phases. While a phase with P63/mmc symmetry had not been previously reported for conventional liquid crystal phases72, we found that both liquid crystal surfactant and silicate phases with symmetry P63/mmc73,21 can be obtained with varying unit cell and cage sizes by using different chain lengths (n) of the form Cn_s_1 over a wide synthesis range (from cell parameter c = 77/~ for C12_3_1 to c = 108/~ for C20_3_1). SBA-2 (below SIP) and SBA-7 (base synthesis) with P63/mmc 3-d hexagonal symmetry are readily synthesized using divalent quaternary ammonium surfactants, Cn_s_1 (e.g., C 12-3-1, C 14-3-1, C16-2-1, C 16-3-1, C 16-6-1, C 18-3-1, C 18-6-1, C20-3-1) in both basic and acidic media. X-ray, AFM and TEM experimental results show that SBA-2 has 3-d hexagonal symmetry, space group P63/mmc (No. 194), and is derived from a hexagonal close packing of globular surfactant/silicate arrays 73. The crystal growth is plate-like and excellent for making thin films and membranes at either an air-water interface 74 or an oil-water interface75 with the sixfold axis normal to the sheet direction. As expected for this geometry, the unit cell parameter c/a ratio is about 1.62. After calcination, the large cage structured mesoporous silica framework remains. The structure directing agent in SBA-2 can be removed by calcination at high temperature (500-600~
This material is thermally stable up to 8000C. The
calcined SBA-2 has a N 2 BET surface area of 500-800 m2g 1. The N 2 adsorption-desorption isotherms is type IV with a H2 hysteresis for even small pore SBA-2 (< 25 A). Thus by systematically varying the surfactant molecular structure as prescribed by the simple packing parameter model, the structural phase space associated with conventional surfactants can be extended to silicate mesoporous structures (Figure 6). Undoubtedly other symmetries and fine details of the nature of the modulated versions of these structures will be forthcoming in the near future.
2.1
M I X E D SURFACTANTS21, 73
The effect of mixing unlike surfactants can be thought of as a simple average of two surfactant packing parameters. For example, a mixture of C16_12_16 and C16_3_1 is used in silicate mesophase synthesis. The products vary from MCM-48 to SBA-2 through MCM-41 as the fraction of C16_3_ 1 increases in the mixture. The mixture of C n-3-1 and CmTMA+ can result in the formation of good quality MCM-41. The MCM-41 easily gives five or more well defined XRD peaks. It is worth noting that high-
15 quality MCM-41 still can be obtained when n = 22, while single surfactant CmTMA § (m > 20) favors the lamellar phases and does not give MCM-41 at 100*C. The high-quality MCM-41 obtained using a mixture of surfactants is thermally stable and the calcined sample still has at least 5 XRD peaks. As for MCM-41 obtained from CnTMA § surfactant, small pore calcined materials are more hydrothermally stable than large pore ones. For example, MCM-41 calcined (at 500~
from
a C12TMA § synthesis system gives a good XRD pattern after 3 hrs heating in water at 100~ while a large pore (-- 55/~) material loses its structure under the same condition. High temperature calcination can increases the hydrothermal stability of these materials. The calcined (at 800~ large pore (~ 55 A) sample shows a clear MCM-41 XRD pattern (5 or more peaks) after 2 hrs heating in water at 100~ When a swelling agent (e.g., TMB) is introduced into this synthesis system, the product MCM-41 has a large unit-cell (dl00 > 60/~) and shows good XRD patterns (4 or more narrow peaks). Our synthesis results indicate the CnTMA § is a good, but not ideal structure directing agent for the formation of MCM-41, even though CnTMA § (e.g., C14TMABr ) itself can give a high quality lyotropic liquid crystal hexagonal phase with five or more sharp reflections 76. CnTMA + has only one charge per hydrophobic chain. More charges (from Cn.3_l, two charges per chain) in the surfactant headgroups apparent are more favorable for the formation of high quality MCM-41. We have found in general for all structural phases that we have investigated that it is possible to fine-tune the synthesis and the quality of the phase even further by using a mixed surfactant approach 73.
2.2 COSOLVENTS
Org an ic c o- s o 1v e n t s are particularly effective in controlling phase
ao
(
palisade ~ \ regi~ FI~-'~'
and interface geometry during the synthesis of both mesoporous inorganic solids 2,3,21,73 and lyotropic mesophases
headgroup
V/aol < 1/3
~ ~
P63/mmc (SBA-2) hydrophobic core
Figure 10 Solvation regions accessible to of surfactant-solvent binary systems77,78. molecules with different dielectric and polar The control comes from being able to properties. The example of g < 1/3 leads to hexagonal close packed geometries. "solvate" the interface head group,
16 palisade and hydrophobic regions associated with the organic surfactant arrays (Figure 10). When a hydrophobic, apolar solvent such as trimethylbenzene is added, it seeks the most hydrophobic region (Figure 11) which is at the tail end of the surfactant array and swells the micelle size. Both V and 1 are affected and the net result can be either a phase change and/or an increase in the effective pore or cage diameter. Thus, when trimethylbenzene (TMB) is added as a swelling agent relatively large pore size changes are observed. This approach has been used in large pore MCM-41 synthesis 2,3,37 and frequently, but not always, works for other mesostructure
phases. C16.3.1 gives SBA-2 (P63/mmc) with a = 62/~, c = 100/~ when TMB/TEOS = 1.1; without TMB, a cell with a = 54/~, c = 87/~ is obtained. In both of these examples, the result is as if a longer chain surfactant (increased 1) has been used to increase the pore size. However, phase changes in some instances are also induced. C16TMA+ favors MCM-41 over a wide range of reactant compositions. At moderately high pH values, if TMB is added, the MCM-41 is replaced by a lamellar phase suggesting that the increased surfactant tail volume is more important. If this lamellar phase sample is heated before silica condensation, it reverts back to the hexagonal trimethylbenzene
configuration 24.
1 increases
A suitable polar additive is able to enter the hydrophobic-hydrophilic palisade region (first
V/aol < 1/3 P63/mmc large cell (SBA-2) Figure 11 Addition of hydrophobic, apolar molecule to surfactant array.
few carbon atoms) of the micelle, with a relative increase in the volume of the hydrophobic core to form surfactant molecule aggregates with a lower curvature surfaces, e.g.,from sphere to rod. Thus when t-amyl alcohol, a polar additive, is added into the synthesis mixture at basic pH, the SBA2 product is replaced by MCM-41 (Figure 12). In the acid synthesis one can make SBA-1 (Pm3n) using C16H33N+(C2Hs) 3 as template without t-amyl alcohol, but SBA-3 (p6m) if t-amyl alcohol is used 21. In our experience the effect of addition of polar solvents is quite predictable and one can very effectively use this to generated desired phases.
~ ~ - ~
t-amyl alcohol increases
i73
J ~
~
Hexagonal (MCM-41)
Figure 12 Phase change from P63/mmc to MCM-41 induced by addition of polar alcohol as solvent
17
2.3 HYDROXY-FUNCTIONALIZED SURFACTANTS The hydroxyl group in the functional surfactant, CnH2n+IN+(CH3)2(CH2)mOH, decreases the hydrophobicity of the headgroup and the headgroup charge is more shielded by water of solvation79 (or silicate or other anions in solution), thus decreasing the affective cationic headgroup area a o. It therefore plays an important role in the entropic and enthalpic contributions of water organization to structure direction. The hydroxyl headgroup surfactants favor formation of mesophases with low surface curvatures such as p6m or lamellar due to the smaller effective a o 37. The product is a lamellar phase when C16H33N+(CH3)2(CH2)2OH is used, while a similar structured surfactant with a smaller headgroup, C16H33N+(CH3)2C2H5, gave only a relatively high surface curvature mesophase, MCM-41. A hydroxyl group in the hydrocarbon chain of the surfactant, e.g., g-substituted, C14H29CH(OH)CH2N+(CH3)3, also has a small effective headgroup surface area. A highly ordered lamellar silicate (to sixth order in Bragg reflections) is obtained by using C14H29CH(OH)CH2N+(CH3)3. In addition, high-angle diffraction peaks are observed that are characteristic of the hydrocarbon chain packing within organized surfactant layer structuresS~
82. The use of zwitterionic surfactants 36 and other functionalized head groups is a
promising area of investigation. 3. INORGANIC CONDENSATION The processes that drive the co-assembly of organic and inorganic units into a bicontinuous composite with spatially distinct organic and inorganic regions of nanostructure are strongly correlated, which
a priori
makes the separation of the various contributing factors difficult to
resolve. Certainly, one would expect that the process of mesophase organization would be strongly coupled to the time-dependent polymerization kinetics of silicate species at the inorganic-organic interface 24. In order to separate the effects of silica polymerization from the thermodynamics of mesophase self-assembly, we have used low temperatures and careful pH control (within 0.1 pH units) to control silica polymerization relative to the overall mesophase assembly. This approach has been used to show that in the absence of inorganic polymerization, these mesophases have liquid crystalline properties, similar to those of conventional aqueous lyotropic liquid crystal systems 24. In order to maintain these liquid crystal-like properties and optimize long range composite ordering during polymerization of the inorganic species, the inorganic and organic domains must
18 be able to reorganize on the same kinetic time scale into mutually compatible configurations. Khushalani et a183 have recently shown that at high temperatures (to 150 ~
and high pH values
(base synthesis mother liquor), one can very nicely get restructuring of the silica phase with a systematic increase in pore size. Under these conditions there is considerable organic thermal disorder, but the kinetic molecular volumes are still effective in generating monodispersed pores. Our approach 21 to optimizing long range ordering and structure has been to maximize the ordering influence of the organic surfactants during the initial polymerization of the silica walls, and then to reduce OI (the organic-inorganic interface interaction) so that the organic and inorganic self assembly are less strongly coupled I
(Figure 13). We chose to do this by 1) using low temperatures to minimize
0.5 to 2
organic disorder and short reaction times
I
hours Iwater 1 powder / o~ | ~product
to kinetically create only partially condensed silica frameworks that can structurally
follow
the
organic
organization and minimize interphase frustration 37, 2) "annealing" the air-dried product at room temperature to further
filter,
as-made sample
air .dry
25~
optimize long range order, and then 3) carrying out the silica polymerization in deionized water (pH -7). The latter greatly reduces the silica charge relative to what it would have in the mother liquor so that
add to H20 at pH - 7
............................. I~ ~7 days, 1 0 0 o c
I =o,., I I -"'" ' a ~ , , , , ~
final product
the organic-inorganic (OI) interactions are correspondingly reduced. This and the
Figure 13 Low temperature, low pH, synthesis of large pore mesostructured phases.
reduced solubility at that pH makes it possible to retain the templating introduced at low temperatures by the more organized organic to the partially polymerized silica. For example, when silicon alkoxides are used as starting reagents at a surfactant-to-silicon ratio o f - 0.1, pH -12, at room temperature or lower, polymerization of the silica begins and a precipitate rapidly forms 37. Silica polymerization of this partly condensed phase is interrupted by using short reaction times (0.5 to 2 hours depending on pH) and then "ripening" the filtered, air dried, solid product at room temperature for 6-10 hours. The solubility of amorphous silica
19
minimizes in water at approximately a pH of 7 to 8, and is more than an order of magnitude less than that at the normal mother liquor pH used in MCM-41 synthesis 84. The X-ray diffraction patterns for a large unit cell (a= 77A calcined) for these MCM-41 phases show seven to eight peaks (Figure 14) and retain their structure on calcination with about a 3% cell shrinkage. N 2 BET measurements reveal that this material has a BJH pore size of 60/~,
Surfactants
5.7 105
22-3-1 + C18TMA+ 100C a = 79.6/~
a pore volume of 1.6 cma/g and a surface O
area of 1086 mE/g. An important feature is that the apparent wall thickness based on
FWHM 0.2 2 0
cps
the absorption isotherm and X-ray data is 17 A,, which is substantially greater than
0
l_2 v,-I
that obtained from conventional MCM-41 synthesis (--8-10/~). This is not surprising in view of the reduced charge associated
01
....
I,,,
2
,k~l~,,~u
3
l-,.,
4
. ! ,_=.~;-~_:--t..
5
6
,
7
8
with the silica phase at the lower pH. Three well-distinguished regions of the adsorption
isotherm
are
noticed:
1.2 106 calcined at 500 C a = 77.0/~
monolayer-multilayer adsorption, capillary condensation, and multilayer adsorption on the outer surface. In contrast to N 2
cps
adsorption results 85,86 of MCM-41 with pore size less than 40/~, a clear type H1 hysteresis
loop
in the
adsorption-
desorption isotherm is observed and the capillary condensation occurs at high relative pressure, consistent with the large pore 87.
0 , ~ .... - : ! . - - . I . . . . 1 2 3 4 5 6 7 8 Figure 14 a) X-ray diffraction pattern after treatment ol room temperature prepared sample at 100 C with wate] at pH 7 and b) after calcination
In all cases that we have examined the treatment improves the structural ordering, however in some cases there is no significant expansion of the unit cell. In the above MCM-41 example, using the indicated mixed surfactants the as made cell has a cell dimension of 54.5/~. Treatment at 2 weeks at 100 ~ in distilled water, pH = 7, gave a cell of 78.2/~, and two additional weeks of treatment gave a cell of 79.6/L However, no significant expansion of the unit cell is observed for MCM-41 and MCM-48 containing a single CnTMA+ molecule, although seven to eight peak
20 diffraction patterns are obtained for the MCM-41 and about twenty peak patterns are generated with MCM-48. The kinetic matching of inorganic and organic ordering during assembly and silica polymerization is critical to the morphological, structural and property design of mesophase materials. 4. INTERFACE CONSIDERATIONS One of the early possible models suggested for mesostructured materials synthesis using surfactants was that of coating preassembled organic arrays with the inorganic phase and then assembling these coated organic arrays into a 3-d periodic structure 88,89. There are features of this model that make it attractive, it gives a direct explanation for the analogous symmetries of the silicate structures to those of liquid crystal chemistry, and it is consistent with what at that time was the paradigm for biomimetic synthesis: first create an organized organic array, and then condense an inorganic phase on the preorganized organic surface 28. At this time, there is convincing evidence 90,91,92 that while stable organized organic arrays are an important part of inorganic nucleation and phase formation in biomineralization, total control by such an array is an extreme condition that is never completely realized. Complete structural phase changes can in fact be induced by soluble proteins 91. Generally, mutually induced structural modifications of the organic and inorganic phases are required to create the higher-order complex microstructures. A more general biomimetic approach must take into account the dynamic balance of solvation, soluble proteins and other soluble organics, organic array assembly, inorganic polymerization and the corresponding interface chemistries. Nevertheless, using pre-organized organics to control morphology and nucleation is a potentially powerful approach to composite materials synthesis, particularly in terms of macroscale shaping, as a template that can be created with the required acid-base or molecular structure characteristics, and as a liquid support phase for bulk processing or synthesis. The concept of using an organized organic array as a template is a statement that the most important free energy and/or kinetic contribution to biphase composite formation is the organization of the organic array. Inorganic deposition and subsequent polymerization do not significantly perturb that array morphology. Several possible ways to approach that goal are 1) to strengthen the organic intraarray coupling by cross-linking; 2) to stabilize the organic array by interfacing it to an inorganic substrate and 3) to decrease the organic-inorganic (OI) interface interactions relative to the organicorganic (O-O) interactions (Figure 2). As far as 3) is concerned, using hydrogen bonding at the interface (Figure 4) rather than
21 ionic or covalent interface interactions (Figure 3) is obviously a step in the right direction. A neutral synthesis route using uncharged (dodecyl amine) or nonionic surfactants (polyethylene oxide) has been explored by Pinnavaia and co-workers93,94 in the near neutral pH range where silica charges on oligomeric silica species (pK a ~ 6 -7) are greatly reduced from that expected at high pH. This is an especially intriguing study since the question of how biosilicates such as diatoms are so exquisitely assembled in nature in this pH region remains unanswered. With neutral surfactants, the primary forces that drive the self assembly of the composite are hydrogen bonding, van der Waals and dipole interactions. Monodispersed porous structures have been obtained in these investigations; however long-range order of the pores is lacking. In this pH regime above the SIP (silica isoelectric point), the silica species are still slightly negatively charged with a relatively high condensation rate. Item 2) above can be achieved by covalent linking to the inorganic substrate 95, so that the patterning of the organic array and the orientation of the organic molecules are defined by the connecting sites to the substrate. In this case the organic array is strongly bound so that its integrity is preserved upon addition of other inorganic phases. Alternatively, cationic organic amphiphiles can be bound to the substrate either by ionic (e.g. mica) or charge
image
and
van
der
Waals
bonding
(graphite) 96,1~ In this case one generates organized, periodic arrays of hemicylinders of CTAB (cetyltrimethylammonium bromide) on graphite and cylinders on mica, in both cases with the long axis of the CTAB organic array parallel to the substrate
Figure 15 Hemicylinders of CTAB formed on graphite. Measurements were made using continuous flow AFM cell with surfactant concentration near CMC 1 concentrations 91.
surface 96 (Figure 15). The advantage of this approach over the covalent attachment of surfactants is clear in that the organic phase is given more freedom and is able to organize in a variety of known liquid crystal geometries. Can these organized organic arrays be used as templates for silica thin film mesostructure nucleation? The answer to this question is yes 97,98, but in the published examples to date only when the mesostructure is formed at pH values below the SIP 36,37 (Figure 4) with the weak OI hydrogen bonding and indirect structure direction. Like the surfactant, silica films prepared on mica have their pore directions oriented parallel to the film surface. Syntheses carried out at high pH values2, 3 are less likely to be successful because of the strong OI interface interactions that can
22 be expected to disrupt the organic array assembly. The divalent surfactants used to create the P63/mmc structures form more stable organic arrays, and are much easier to convert into mesostructured films, even at basic pH values 74. The same situation applies to oriented thin silica films prepared at the air-water interface. Beautiful flexible sheets of periodic mesostructured films with p6m or subgroup symmetry (SBA-3) and the channels parallel to the film plane are formed with silica chemistry carried out at pH values below the SIP 99, but similar thin films of the MCM-41 phase have not so far been successfully made at basic pH values. Similarly, Attard and co-workers attempts to use liquid crystal structural phases formed in concentrated solutions of surfactants as templates required low pH values below SIP 100. In these examples the mechanism does not necessarily involve the simple coating of the organic array, since the hydrolysis of the silicon alkoxide used as a precursor may change or initially disrupt the organic phase structure. The important point however, is that with a weakly interacting inorganic-organic interface, the thermodynamic and kinetic factors that gave the original organic assembly its structural properties are still dominant and can control the composite organization. It should be emphasized that the acid(below SIP) and base synthesized silica mesophases have little in common other than sometimes the same space group symmetry. They do not have the same composition since mesophase samples synthesized below the silica isoelectric point require a counter anion, generally a halide anion, for each surfactant molecule that is present. Terminal Si-Ogroups are protonated so that the bulk compositions of M41S and acid prepared materials (APM) made with the same surfactants are completely different in hydrogen and halide ion content. The ion-pair surfactants of the APM materials are readily removed by washing with distilled water/ethanol at --70 ~
since the wall charge is neutral or slightly positive. Removal of
surfactant from M41S samples requires ion exchange by refluxing with acidic ethanol because of the negatively charged terminal oxygen atoms. Absorption and desorption properties similarly differ substantially. The ultimate periodic symmetry is determined in both cases by the nanophase surfactant packing requirements, so that similar space group and lattice symmetries may be observed by x-ray diffraction transmission electron micrographs. However the Bragg peaks of the two phases for a given surfactant have clearly different diffraction intensities, indicating different pore and wall structure. As pointed out by Brinker and Scherer 101, silica hydrolysis below SIP results in Huggins or chain like polymerization while M41S silica polymerization conditions lead to Einstein or cluster
23 like configurations with extensive cross-linking so that different silica wall structures are expected for the acid and base synthesized structures. The difference in wall and pore structure is evident in BET absorption isotherm measurements that show that APM exhibit a very different sorption behavior from M41S samples with a step in the isotherm at appreciably lower P/P0 values (p, pressure) than samples synthesized from alkaline media with a similar lattice spacing. These data and diffraction results show that the acid silica walls are effectively thicker than those of the corresponding M41S phases prepared at pH values above 10. Nevertheless, BET surface areas calculated for such samples can be a factor of two higher, indicating the presence of micropores or highly ruffled pore surfaces. Even taking into account the limitations of BET analysis for such materials, the difference in the values obtained indicates a major difference in the pore and wall structure of APM and MCM-41 type materials.
5. MACROSCALE STRUCTURES WITH PERIODIC MESOPORES75,102 Organic-inorganic hybrids are ubiquitous in nature as biominerals and inherently offer many opportunities for the creation of new materials with unusual features. As diphasic structures, they can be made shaped and multifunctional. The key to the integration of the organic and inorganic components is to use low temperature chemistry to control the kinetics of assembly of the organic and inorganic components, and an integral part of that process lies at the interface between the spatially distinct organic and inorganic regions. The extent to which the organic and inorganic domains have properties and structure that are characteristic of the corresponding bulk phases depends on the strength of the interface inorganic-organic (IO) interaction. The significance of this in hybrid organic-inorganic materials design has been recognized by Clement 103, who divides hybrid organic-inorganic materials into two distinct classes. In Class I, only weak bonds (e.g., hydrogen, van der Waals) give cohesion to the whole structure. In Class II the organic and inorganic components are linked together by strong chemical bonds (e.g., covalent or ionocovalent bonds). This differentiation is fundamental to the property design of organic-inorganic hybrid materials for a wide range of applications. The differences in the properties of the mesostmctured silica phases that are generated by base synthesis, an example of Class II (Figure 3) organic/hybrid materials, from the Class I silica mesostructures made at pH values below the aqueous silica isoelectric point (Figure 4) support this view. As another example of how weak OI interactions can be applied to materials synthesis, we have used the combination of long-range oil-in-water emulsion and oil-water interface physics with shorter-range molecular assembly of silica and surfactants at the emulsion interface to create
24 ordered composite mesostructured phases that are also macroscopically structured and shaped75,102. Microemulsions and emulsions occupy a special place in the hierarchy of structures, in that their formation involves long-range forces with an energy of assembly, including shape fluctuations and interaggregate interactions, about the same as the thermal energy kT 104. Hydrodynamic, long-range forces can therefore be used to define emulsion morphology and the configuration of the emulsion oil-water interface. With self-assembly energies approaching kT, emulsions are often close to the limit of stability. In order to stabilize the emulsion phase, current commercial practice is to use surfactants. Thus, oil-in-water emulsions are stabilized by short range (10 -7 m), and relatively weak van-der Waals interactions between the hydrophobic tails of amphiphilic surfactants and the emulsion organic phase. This combination provides an ideal starting place for periodic mesostructured inorganic phase synthesis. If an oil-in-water interface is used as an inorganic growth medium with the growth direction into the aqueous phase, morphological control of the resulting inorganic/organic composite assembly can be achieved at micron and longer length scales. The morphology of the preorganized organic liquid phase is preserved during the periodic mesopore synthesis by working at acid pH below the SIP, making use of the weak organic-inorganic interactions shown in Figure 4 (S§
+ structure directing during synthesis).
Mesoporous silica fibers, diatom-like hollow
spheres, and thin films are some of the morphologies that have been synthesized using conventional emulsion hydrodynamics, p6m, P63/mmc and Pm3n wall structures can be made. Surface areas of the calcined products are greater than 1000 m2/gm with narrow pore distributions. The results are of interest with regard to packaging, perhaps in slow-release applications. Hydrodynamics and emulsion technology are highly advanced commercially and the connection of this to inorganic/organic hybrid materials synthesis presents new process possibilities for hierarchically structured composite phases. 6. S U M M A R Y
As indicated in the Introduction, the discovery of periodic mesoporous structures is a major advance in composite organic-inorganic materials synthesis. In the short presentation given here, much has been omitted concerning our growing knowledge in this very rapidly expanding field, but hopefully it is clear that the organic and inorganic phases can be synergistically integrated in a pre-designed fashion. It also seems possible to carry out this co-assembly of organic and inorganic species using fluid mechanics to define macroscale shapes. Of particular interest are the
25 increasingly sophisticated studies of the dynamic processes and organic-inorganic interfaces that are present in biomineralization. These investigations seem to be converging with those being made on synthetic hybrid organic-inorganic materials, and the result could be an even more rapid evolution of technological applications. The confluence of these two trains of thought is certain to enhance an already exciting era in materials synthesis. REFERENCES
1. Yanagisawa, T.; Shimizu, T.; Kuroda, K.; Kato,C. Bull. Chem. Soc. Jpn., 1990, 63, 988. 2. Kresge, C.T.; Leonowicz, M.E.; Roth, W.J.; Vartuli, J.C.; Beck, J.S. Nature, 1992, 359, 710. 3. Beck, J.S.; Vartuli, J.C.; Roth, W.J.; Leonowicz, M.E.; Kresge, C.T.; Schmitt, K.T.; Chu, C.T-W.; Olson, D.H.; Sheppard, E.W.; McCullen, S.B.; Higgins, J.B.; Schlenker, J . L . J . Am. Chem. Soc., 1992, 114, 10834. 4. Vartuli, J.C.; Schmitt, K.D.; Kresge, C.T.; Roth, W.J.; Leonowicz, M.E.; McCullen, S.B.; Hellring, S.D.; Beck, J.S.; Schlenker, J.L.; Olson, D.H.; Sheppard, E.W. Chem. Mater., 1994, 6, 2317. 5. Vartuli, J.C.; Kresge, C.T.; Leonowicz, M.E.; Chu, A.S.; McCullen, S.B.; Johnson, I.D.; Sheppard, E.W. Chem. Mater., 1994, 6, 2070. 6. Beck, J.S.; Vartuli, J.C.; Kennedy, G.J.; Kresge, C.T.; Roth, W.J.; Schramm, S.E. Chem. Mater., 1994, 6, 1816. 7. Flanigen, E.M.; Patton, R.L.; Wilson, S.T. Stud. Surf Sci. Catal., 1988, 37, 13. 8. Zones, S.I.; Olmstead, M.M.; Santilli, D.S.J. Am. Chem. Soc., 1992, 114, 4195. 9. Davis, M.E.; Lobo, R.F. Chem. Mater., 1992, 4, 756. 10. Harris, T.V.; Zones, S.I., in Zeolites and Related Microporous Materials: State of the Art 1994; J. Weitkamp, H.G. Karge, H. Pfeifer, and W. Holderich, Eds.; Elsevier: Amsterdam, 1994, p. 29. 11. Shimizu, A.; Taniguchi, Y., Bull. Chem. Soc. Jpn., 1990, 63, 1572 and 3255. 12. Davis, M.E.; Zones, S.I., in Synthesis of Microporous Materials: Zeolites, Clays and Nanostructures, M.L. Occelli and H. Kessler, Eds.; Marcel Dekker, New York, 1996. 13. Helmkamp, M.M.; Davis, M.E. Ann. Rev. Mater. Sci., 1995, 25, 761. 14. Petrovic, I.; Navrotsky, A.; Davis, M.E.; Zones,S.I. Chem. Mater., 1993, 5, 1805. 15. Burkett, S.L.; Davis, M.E., Chem. Mater., 1995, 7, 1453 and included references. 16. Nakagawa, Y. Stud. Surf. Sci. Catal., 1995, 97, 53. 17. Kubota, Y.; Helmkamp, M.M.; Zones, S.I.; Davis, M.E. Microporous Materials, 1996, 6, 213. 18. Mallouk, T. J. Am. Chem. Soc., 1994, 116, 8374. 19. Mallouk, T. Acc. Chem. Res., 1992, 25, 420. 20. Stucky, G.D. et al. Abstract, Symposium on Access in Nanoporous Materials, Michigan State University, East Lansing MI, June 1995. 21. Huo, Q.; Margolese, D.I.; Stucky, G.D., Chem. Mater. 1996, 8,1147. 22. Burkett, S.L.; Sims, S.D.; Mann, S. Chem. Commun., 1966, 1367. 23. Firouzi, A.; Kumar, D.; Bull, L. M.; Besier, T.; Sieger, P.; Huo, Q.; Walker, S. A.; Zasadzinski, J.; Glinka, A.C.; Nicol,J.; Margolese, D.; Stucky, G.D.; Chmelka, B.F. Science, 1995, 267, 1138.
26 24. Firouzi, A.; Stucky, G.D.; Chmelka, B.F. Synthesis of Microporous Materials, M.L. Occelli and H. Kessler, Eds., Marcel Dekker (in press). 25. Antonelli, D.M.; Ying, J.Y. Angew. Chem. Int. Ed. Engl. 1995, 34, 2014. 26. Weiner, S. Crit. Rev. Biochem., 1986, 20, 365. 27. Weiner, S.; Traub, W. Phil. Trans. Royal Society of London, 1984, B304, 428. 28. Mann, S.; Archibald, D.D.; Didymus, J.M.; Douglas, T.; Heywood, B.R.; Meldrum, F.C.; Reeves, N.J. Science, 1993, 261, 1286. 29. Mann, S. Nature, 1993, 365, 499. 30. Archibald, D.D.; Mann, S. Nature, 1993, 364, 430. 31. Heywood, B.R.; Mann, S. Adv. Materials, 1994, 6, 9. 32. Baral, S.; Schoen, P. Chem. Mater, 1993, 5, 145. 33. Archibald, D. D.; Mann, S. Nature, 1993, 364, 430. 34. Bunker, B.C.; Rieke, P.C.; Tarasevich, B.J.; Campbell, A.A.; Fryxell, G.E.; Graff, G.L; Song, L.; Liu, J.; Virden, J.W.; McVay, G.L. Science, 1994, 264, 48. 35. This notation refers to the solution species used in the synthesis, S = surfactant or surfactant precursor, X = the acid anion which is usually C1-or Br- in syntheses carried out below the aqueous silica isoelectric point (SIP) (pH ~2), and I§ or I- is used to designate the charge of the solution inorganic species that are present. Neutral silica species are also present, with a concentration that varies with pH; however in our experience the condensation rate and the quality of the mesostructure that is formed varies inversely with the neutral silica concentration in the pH region immediately below the SIP. 36. Huo, Q.; Margolese, D.I.; Ciesla, U.; Feng, P.; Gier, T.E.; Sieger, P.; Leon, R.; Petroff, P.M.; Schtith, F; Stucky, G.D. Nature, 1994, 368, 317. 37. Huo, Q.; Margolese, D.I.; Ciesla, U.; Demuth, D.G; Feng, P.; Gier, T.E.; Sieger, P.; Chmelka, B.F; Schtith, F; Stucky, G.D. Chem. Materials, 1994, 6, 1176. 38. Yange, H.; Kupermann, A.; Coombs, N.; Mamiche-Afara, S.; Ozin, G. Nature, 1996, 379, 703. 39. Yang, H.; Coombs, N.; Sokolov, I.; Ozin, G.A. Nature, 1996, 381,589. 40. Attard, G.S.; Glyde, J.C.; Goltner, C.G. Nature,1995, 378, 366. 41. Tiddy, G.J.T. Physics Reports, 1980, 57, 1 42. Luzzati, V.; Vargas, R.; Mariani, P.; Gulik, A.; Delacroix, H. J. Mol. Biol., 1993, 229, 540. 43. Henriksson, U.; Blackmore, E.S.; Tiddy, G.J.T.; Soderman, O. J. Phys. Chem., 1992, 96, 3894. 44. Husson, F.; Mustacchi, H.; Luzzati, V. Acta Crystallogr., 1960, 13, 668. 45. Hagslatt, H; Soderman, O; Jonsson, B. Liquid Crystals, 1994, 17, 157. 46. Jahns, E.; Finkelmann, H. Colloid Polymer Sci., 1987, 265, 304. 47. Hagslatt, H.; Soderman, O.; Jonsson, B. Langmuir, 1994, 10, 2177. 48. Kratzat, K.; Finkemann, H. Colloid & Polymer Science, 1994, 272, 400. 49. Gulik, A.; Delacroix, H.; Kirschner, G.; Luzzati, V. J. Phys. H, 1995, 5, 445. 50. Hyde, S.T. Pure and Applied Chemistry, 1992, 64, 1617. 51. Hyde, S.T.J. Phys. Chem., 1989, 93, 1458. 52. Monnier, A.; Schtith, F; Huo, Q.; Kumar, D; Margolese, DT; Maxwell, R.S.; Stucky, G.D.; Krishnamurty, M.; Petroff, P.; Firouzi, A.; Janicke, M.; Chmelka, B.F. Science, 1993, 261, 1299. 53. Stucky, G.D.; Monnier, A.; Schtith, F.; Huo, Q.; Margolese, DT; Kumar, D.; Krishnamurty, M.; Petroff, P.; Firouzi,A.; Janicke, M.; Chmelka, B.F. Mol. Cryst. Liq.Cryst., 1994, 240, 187. 54. Alfredsson, V.; Anderson, M. W. Chem. Mater, 1996, 8, 1141.
27 55. Gruner, S.M.J. Phys. Chem., 1989, 93, 7562. 56. Landry, C.C.; Stucky, G.D., submitted for publication. 57. Garc6s, J.M. Adv. Mater., 1996, 8, 434. 58. Khushalani, D.; Kuperman, A.; Ozin, G.A.; Tanaka, K.; Garces, J.; Olken, M.M.; Coombs, N. Adv. Mater., 1995, 7, 1156. 59. Israelachvili, J.N.; Mitchell, D.J.; Ninham, B.W. J. Chem. Soc., Faraday 2, 1976, 72, 1525. 60. Israelachvili, J.N.; Mitchell, D.J.; Ninham, B.W. Biochim. Biophys. Acta, 1977, 470, 185. 61. Fogden, A.; Hyde, S.T.; Lundberg, G. J. Chem. Soc., Faraday Trans., 1991, 87, 949. 62. Huo,Q.; Stucky, G.D. Materials Research Society Meeting, San Francisco, April 1996. 63. Preliminary modelling was done in collaboration with MSI and Biosym, John Newsam and Clive Freeman. 64. Sadoc, J.F., et al., J. Phys. France, 1988, 49, 52. 65. Gies, H. Zeit. Kristallogr., 1983, 164, 247. 66. Alami, E.; Beinert, G.; Marie, P.; Zana, R. Langmuir,1993, 9, 1465. 67. Menger, F~M.; Littau, C.A.J. Am. Chem. Soc., 1993, 115, 10083. 68. Alami, E.; Levy, H.; Zana, R. Langmuir, 1993, 9, 940. 69. Zana, R.; Talmon, Y. Nature, 1993, 362, 228. 70. Danino, D.; Talmon, Y.; Zana, R. Langmuir, 1995, 11, 1448. 71. Zana, R.; Benrraou, M.; Rueff, R. Langmuir, 1991, 7, 1072. 72. During the writing of this manuscript an article (M. Clerc_"A New Symmetry for the Packing of Amphiphilic Direct Micelles") that describes Pm 3 n and P63/mmc phases for the C12EOs/water binary system appeared in J. Phys. H France, 1996, 6, 961. 73.Huo, Q." Leon, R.; Petroff, P.M.; Stucky, G.D. Science, 1995, 268, 1324. 74.Tolbert, S.; Huo, Q.; Stucky, G.D., submitted for publication. 75.Schacht, SI,~ Huo, Q." Voigt-Martin, I.G.; Stucky, G.D." Schtith, F. Science, August 199~ 76.McGrath, K.M. Langmuir, 1995, 11, 1835. 77.DeLisi, R.; Milioto, S. Chem. Soc. Rev., 1994, 23, 67. 78.Rosen, M.J. Surfactants and Interfacial Phenomena (Wiley-Interscience,New York, 1989). 79.Zana, R.; Levy, H. J. Colloid lnterface Sci. 1995, 170, 128. 80. Harlos, K. Biochim. Biophys. Acta, 1978, 511, 348. 81.Janiak, M.J.; Small, D.M.; Shipley, G.G., Biochemistry, 1976, 15, 4575. 82.Watts, A.; Harlos, K.; Marsh, D., Biochim. Biophys. Acta, 1981, 645, 91. 83. Khushalani, D.; Kuperman, A; Ozin, G.A.; Tanaka, K.; Garces, J.; Olken, M.M.; Coombs, N. Adv. Mater. 1995,7,842. 84. Iler, R.K., "The Chemistry of Silica", John Wiley and Sons, NY, 1979, p 42. 85. Schmidt,R.; Hansen,E.W.; Stocker,M.; Akporiaye,D.; Ellestad,O.H., J. Am. Chem. Soc., 1995, 117, 4049. 86.Branton,P.J.; Hall,P.G.; Sing,K.S.W.; Reichert,H.; Schuth,F.; Unger,K.K., J. Chem. Soc. Faraday Trans., 1994, 90, 2965. 87. Llewellyn,P.L.; Grillet,Y.; Schuth,F.; Reichert,H.; Unger,K.K., Microporous Mater., 1994, 3, 345. 88. Chen, C.; Li, H.; Davis, M.E. Microporous Materials, 1993, 2, 17. 89. Chen, C.; Burkett, S.L.; Li, H.; Davis, M.E. Microporous Materials, 1993, 2, 27. 90.Belcher, A.M.; Wu, X.H.; Christensen, R.J.; Hansma, P.K.; Stucky, G.D.; Morse, D.E. Nature, 1996, 381, 56. 91. Zaremba, C.M.; Belcher, A.M.; Fritz, M.; Li, Y.; Mann, S.; Hansma, P.K.; Morse, D.E.;
28 Speck, J.S.; Stucky, G.D. Chem. Mater., 1996, 8, 679. 92. Falini, G. et al., Science, 1996, 271, 67. 93. Tanev, P.T.; Pinnavaia, T.J. Science, 1995, 267, 865. 94. Bagshaw, S.A.; Prouzet, E.; Pinnavia, T.J. Science, 1995, 269, 1242. 95. Bunker, B.C.; Rieke, P.C.; Tarasevich, B.J.; Campbell, A.A.; Fryxell, G.E.; Graff, G.L.; Song, L.; Liu, J.; Virden, J.W.; McVay, G.L. Science, 1994, 48. 96. Manne, S.; Cleveland, J.P.; Gaub, H.E.; Stucky, G.D.; Hansma, P.K. Langmuir, 1994, 10, 4409. 97. Yang, H.; Kuperman, A.; Coombs, N.; Mamiche-Afara, S.; Ozin, G.A. Nature, 1996, 379, 703. 98. Aksay, I.A., et al., Materials Research Society Meeting; Boston, Massachusetts, November 1994; European Science Foundation Symposium on Biomineralization; Granada, Spain, September 1995; International Symposium on Synergistic Synthesis of Inorganic Materials, Tagungsst~itte Schloss Ringberg der Max-Planck-Gesellschaft, March 1996. 99. Yang, H.; Coombs, N.; Sokolov, I .; Ozin, G.A. Nature, 1996, 381,589. 100. Attard, G.S.; Glyde, J.C.; G61tner, C.G. Nature, 1995, 366. 101. Brinker, C.J.; Scherer, G.W.J. Non-cryst. Solids, 1985, 70, 301. 102. Schacht, S., Diploma Thesis, Mainz, 1995. 103. Sanchez, C.; Ribot, F. New. J. Chem., 1994, 18, 1007. 104. Israelachvili, J. Colloids and Surfaces A: Physicochemical and Engineering Aspects 1994, 91, 1. 105. Manne, Srinivas; Gaub, Hermann E. Science,1995, 270, 1480.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
29
Incorporation and Stability of Trivalent Cations in Mesoporou_s Silicas Prepared using Primary Amines as Surfactant S. Gontier and A. Tuel Institut de Recherches sur la Catalyse. C.N.R.S. 2, av. A. Einstein 69626 Villeurbanne Cedex France
Abstract A series of trivalent metal (A13+, Ga 3+, Fe 3+, B 3+) containing mesoporous silicas (Me-MS) have been synthesized using hexadecylamine as organic templating surfactant. All materials possess mesopores of about 37/~ diameter and surface areas above 900 m2/g. A solvent extraction has been used to remove the template from the solids. As compared to a conventional thermal treatment, this procedure preserves the mesopore structure and the coordination of the cations. Extracted samples are thermally stable and can be calcined in air at high temperature without observing changes in the cation coordination.
1. I N T R O D U C T I O N The family of silica-alumina based mesoporous molecular sieves M41S has received considerable interest over the last years because of their praticularly attractive characteristics like very high surface areas and regular mesopores whose diameter can be varied between 20 and 100/~ [1]. MCM-41, the well-known hexagonal member of this family is usually prepared with cetyltrimethylammonium (CTMA) cations and possesses mesopores in the 35-40/~ range [2]. As for zeolites, several trivalent cations can be incorporated in MCM-41, whose composition can be varied within a quite large domain of Si/Me ratios. Recently, Tanev et al. [3] have reported the synthesis of Hexagonal Mesoporous Silicas (HMS) by a neutral templating route using primary alkylamines in C 8 to C18 as surfactant. These materials are very similar to pure silica MCM-41, but differ by the arrangement of the mesopores. The neutral templating route offers several advantages with respect to the conventional preparation using ammonium cations. In particular, the synthesis is performed at room temperature and the template can be removed by ethanol extraction. The removal of organics by solvent extraction is not only interesting from an environmental point of view but it also preserves the mesoporosity of the samples, which is not always the case upon thermal treatment at high temperature
[3].
30 In the present paper, we report the synthesis of various trivalent cations (A13 +, Ga 3+, Fe 3+ and B3+) containing mesoporous silicas using hexadecylamine as surfactant. Template-free materials were obtained either by calcination in air at 650~ or by a solvent extraction. The influence of both procedures on the preservation of the mesoporosity and on the nature of the trivalent metal coordination is discussed.
2. E X P E R I M E N T A L In a typical synthesis, a solution containing 1 tool of tetraeth)~l' orthosilicate (TEOS), 6.5 mol of ethanol and 1 tool of isopropyl alcohol is mixed to a second solution containing 0.3 tool of hexadecylamine in 36 mol H20. Depending on its nature, the trivalent metal precursor is introduced either in the first solution (aluminium isopropoxide, tributyl borate) or with the amine (aluminium nitrate, gallium nitrate, iron nitrate or boric acid). The gel is vigorously mixed at room temperature for about 30 min and aged under static conditions for 12 h. The solids are then recovered, washed abundantly with distilled water and air-dried. For the solvent extraction of the organics, 1 g of dried solid is dispersed in 100 ml ethanol containing 1 g NaC1 and the suspension is refluxed for 1 h. The template-free samples are then dried at 80~ for 12 h. Samples are characterized using X-ray diffraction (CGR Theta 60 diffractometer using Cu Ka radiation), N 2 adsorption/desorption (Catasorb apparatus) and Solid State NMR (Bruker MSL 300). EPR spectra are obtained on a Varian E9 spectrometer. Chemical analysis are performed by atomic absorption after solubilization of the samples in HF-HC1 solutions.
3. RESULTS AND DISCUSSION The chemical composition of the various samples is given in Table 1. For all samples (except B-containing materials) the amount of metal in the solid corresponds approximately to that introduced in the synthesis gel. As a general trend, the yield in solid decreases with the metal content. The case of boron is interesting as it is the single example where the boron content is lower in the solid than in the gel, particularly for samples prepared with low Si/B ratios. Moreover, it is possible to prepare samples with low Si/B ratios in relatively high yields. Comparison of samples 1 and 2 or 14 and 15 shows that the nature of the precursor does not greatly influences the metal content in the final product. The maximum metal incorporation-is approx, the same for A1, Ga and Fe and corresponds to Si/Me ratios of about 10 in the solid phase. When syntheses are performed with lower ratios in the gel, the yield in solid is usually very low and spectroscopic characterization shows that as-synthesized samples contain non-framework octahedrally coordinated species.
31 Table 1 Chemical composition of the different samples Si/Me No
Sample
Gel
Product
Yield (%)
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19
A1-MS(100) A1-MS(100) a A1-MS(50) A1-MS(20) A1-MS(15) Ga-MS(100) Ga-MS(50) Ga-MS(20) Ga-MS(15) Fe-MS(100) Fe-MS(50) Fe-MS(20) Fe-MS(15) B-MS(100)_ B-MS(100) ~ B-MS(50) B-MS(15) B-MS(3) B-MS(l)
100 100 50 20 15 100 50 20 15 100 50 20 15 100 100 50 15 3 1
88 97 38 21 8 86 48 14 13 85 55 18 15 150 166 95 27 17 7
86 89 85 63 50 92 83 56 30 89 81 63 48 86 88 82 97 96 81
aThe sample was prepared with aluminium ethoxide, bThe sample was prepared using boric acid. As-synthesized samples are characterized by a single broad X-ray line around 2.2 ~ (20), as already reported for HMS [4]. After calcination in air at 650 C, all samples exhibit high surface areas but Horvath-Kawazoe pore size distributions show that the mesopore system partially collapses upon thermal treatment, particularly for samples containing high metal contents (Table 2). This was also confirmed by X-ray diffraction. Solid state NMR characterization of as-synthesized samples shows that A13+, Ga 3 + and B 3 + are tetrahedrally coordinated, at least for samples with Si/Me > 10. For low A1 contents, spectra of both as-synthesized and calcined samples show a single line at-about 52 ppm, as already reported for MCM-41 [5] (Fig. 1). For high A1 contents, the spectra of calcined samples show an additional peak around 0 ppm attributed to octahedrally coordinated A1 species resulting from a partial removal of framework aluminium. This removal probably occurs during the collapse of the mesopore structure.
32 Table 2 Characteristics of various samples Si/Me No
Sample
Gel
Product
S(m2/g)
~p(/~)a
1 4 5 7 11 14 17 18
AI-MS(100) AI-MS(20) AI-MS(15) Ga-MS(50) Fe-MS(50) B-MS(100) B-MS(15) B-MS(3)
100 20 15 50 50 100 15 3
88 21 8 48 55 150 27 17
1215 (1166) 983 (1079) 1252 929 700 (935) (1056) 1237 (935)
30 (36) 32 (37) 22 28 22 (37) (36) 30 (38)
,
a~p is the pore diameter obtained from N 2 isotherms. Valuesbetween parentheses have begn obtained on solvent extracted samples.
52
52
I
A (
CALCINATION
I
~ 650~
m
"
o-'
o'
, 6o
5 0'
o' - 5 0
ppm/Al(H20]8 s§ Fig. 1 27A1 NMR spectra of samples 1 (a) and 4 (b) before (left) and after (right) calcination in air
The 11B NMR spectra of B-MS materials show a single line at -1.5 ppm, characterisitc of B3+ in tetrahedral sites [6]. Upon calcination, the spectrum is modified and a second resonance, assigned to BO 3 units, is observed (Fig. 2). The 71Ga NMR spectra of Ga-MS materials show a broad line at 167 ppm, already observed on Ga-containing zeolites and assigned to tetrahedrally coordinated Ga species [7]. The EPR spectra of FeMS solids are very similar to those obtained on Fe-containing zeolites and show a sharp peak at -~+ge-- 4.3 usually attributed to F cations in a tetrahedral coordination [8].
33
-1.5
I
= 0.24
6
I
_
-
-
-
~
.
.
.
.
(b)
(a)
40'
'
2 "0
'
0'
. - 2. 0 . . - 4 0
ppm/Et2OBF3
Fig. 2. 11B NMR spectra of sample 18 as-synthesized (a) and calcined (b).
'60
-8
-100 -1 0 ppm/TMS
-140
Fig. 3. 29Si NMR spectra of sample 3. As-synthesized (a), extracted (b) and calcined in air (c)
29Si MAS NMR spectra of as-synthesized samples show 3 distinct lines at -90, -98 and -110 ppm, attributed to Q2, Q3 and Q4 species, respectively. After calcination, the spectrum is less well resolved and a deconvolution shows that approx. 50 % of the silanol groups have been removed with respect to as-synthesized products (Fig. 3). For pure silica materials, Tanev et al. [3] have reported that washing the mesoporous silica with boiling ethanol resulted in the total removal of the amine from the mesopores. That could be possible because of the weak interactions (hydrogen bonding) between the neutral organic micelle system and the inorganic framework. However, when trivalent cations are tetrahedrally coordinated in a silica matrix, they create a defect charge that has to be compensated by cations. When no cations are present in the gel, the charge is balanced by templating molecules, usually tetraalkyla .mmonium cations. We have first followed that recipe, i.e. the dried samples were refluxed in ethanol for about 1 h. The procedure removes nearly all the organics, as evidenced by the strong decrease of specific absorption bands in i.r. spectra. However, absorptions characteristic of the template are still present in the i.r. spectrum after 3 ethanol extractions. The 13C
34 NMR spectrum of the extracted sample is quite similar to that of as-synthesized samples but shows additional bands, particularly one at 41 ppm/TMS, attributed to carbon atoms directly bonded to primary ammonium cations [9]. These cations, that are not removed by ethanol extraction, are more likely in the proximity of Me 3+ cations and serve to maintain the electric neutrality of the samples. Therefore, the incorporation of trivalent cations in mesoporous silicas necessitates the protonation of a small amount of the primary amine. We thus tried to add inorganic cations to the extraction solvent to exchange primary ammonium cations. The procedure was similar to that previously described except that NaC1 was preliminary dissolved in ethanol (lg/100 ml). I.r. and NMR spectroscopies show that all organics are then removed, even in samples containing high metal contents. However, new absorptions are observed in the i.r. spectrum around 2900 cm -1, characteristic of Si-O-C2H 5 species formed after partial esterification of the samples, which was confirmed by a significant decrease of the OH band at 3745 cm "1. Chemical analysis of the samples show that the extraction does not modify the composition of the samples. After removal of the template, all samples exhibit high surface areas and pore sizes of about 37,1. (Table 2). 52
i
(~
1
I
50
I
0
I
-50
ppm / AI (H20)O*
Fig. 4. 27A1 NMR spectra of sample 4. As-synthesized (a), calcined in air (b), extracted (c) and extracted and calcined in air at 500~ (d).
35 Fig. 4 compares the 27A1 NMR spectra of sample 4 as-synthesized, calcined at 650~ in air and submitted to the solvent extraction. As clearly demonstrated in the figure, the solvent extraction preserves the coordination of AI3+ , as n o octahedrally coordinated species are detected. The spectrum is very similar to that of the assynthesized sample. Moreover, the spectrum is unchanged when the solvent extracted sample is submitted to a calcination in air at 500 ~ which confirms that-the formation of octahedrally A1 species more likely occurs during the decomposition of the organics at high temperature. Similarly, the liB NMR spectra of solvent extracted B-MS samples are very different from those of the corresponding calcined samples (Fig. 5).
-1.5
I
'
40
I
20
I
0
I
!
-20
-40
.
ppm/Et2OBF 3
Fig. 5. llB NMR s~ectra of sample 18. As-synthesized (a), extracted (b) and extracted and calcined at 500 C in air (c).
Only one line is observed, as for as-synthesized samples, and characterizes B(OSi)4 units. As for aluminium containing materials, a subsequent calcination does change the NMR spectrum. EPR spectroscopy shows that the solvent extraction also preserves the coordination of Fe 3 + cations in mesoporous silicas. EPR spectra are identical to those of as-synthesized samples and not modified by a subsequent calcination in air.
36 The 29Si NMR spectra of solvent extracted samples are strictly similar to those of as-synthesized samples (Fig. 3). The fraction of silanol groups are the same as for starting materials, thus confirming once more the preservation of the framework. However, a small amount of the species observed around -100 ppm are probably Si-OC2H 5 moities due to the partial esterification of silanol groups during the extraction.
4. CONCLUSION We have shown that trivalent metal containing mesoporous silicas could be prepared using a primary amine as surfactant molecule. The physical properties of the materials, in particular their surface area, did not significantly change with the amount of metal incorporated. Following this recipe, mesoporous silicas containing tetrahedrally coordinated cations could be synthesized with Si/Me ratios as low as 10 without observing the presence of octahedral species. The totallity of the organics could be removed from the mesopores using a solvent extraction. The procedure preserved not only the mesoporosity of the materials but also the coordination of the trivalent cations. Extracted samples were thermally stable and could be calcined in air at 500~ without modification of the cation coordination. This calcination had the advantage to remove ethoxy groups bonded to the silica framework and formed upon the extraction process.
5. R E F E R E N C E S
C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli ande J.S. Beck, Nature, 359 (1992) 710. J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T-W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins and J.L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. P.T. Tanev and T.J. Pinnavaia, Science, 267 (1995) 865. P.T. Tanev, M. Chibwe and T.J. Pinnavaia, Nature, 368 (1994) 321. A. Corma, V. Fornes, M.T. Navarro and J. Perez-Parient6, J. Catal., 148 (1994) 569. A. Sayari, I. Moudrakovski, C. Danumah, C.I. Ratcliffe, J.A. Ripmeester and K.F. Preston, J. Phys. Chem, 99 (1995) 16373. Y.X. Zhi, A. Tuel, Y. Ben Taarit and C. Naccache, Zeolites, 12 (1992) 138. D.H. Lin, G. Coudurier and J.C. Vedrine, in P.A. Jacobs and R.A. Van Santen (Eds), Zeolites: Facts, Figures and Future, Elsevier Science Publishers, B.V. Amsterdam, 1989, p. 1431. G. Boxhoonn, R.A. Van Santen, W.A. Van Erp, G.R. Hays, N.C.M. Alma, R. Huis and A.D.H. Clague, Proc. 6th Int. Zeolite Conf. (Reno, 1983), Butterworth, Guilford, 1985, p. 694.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
37
Synthesis of lamellar aluminophosphates via the supramolecular templating mechanism Abdelhamid SAYARI Department of Chemical Engineering and CERPIC, Universit~ Laval, Ste-Foy, Qc, Canada G1K 7P4. The liquid-crystal templating approach for the synthesis of mesostructured materials was extended to aluminophosphates. Long chain primary and tertiary amines were used as templates. The molar gel composition was varied in a systematic manner over a wide range. Samples were thoroughly characterized using XRD, TEM, TGA, and 3~p, 27AI, 15N and lsC solid state NMR. Several lamellar phases with doo~distances in the 2 to 4 nm range were obtained. However, no three dimensional structures were detected. The gel composition was found to have a strong effect on the connectivity of aluminum and phosphorus in the final "crystalline" phase, as well as on their doo~ distances. TEM showed that some samples exhibit extended areas with unique structural features. They consisted of coaxial cylinders of alternating inorganic aluminophosphate material and organic surfactant bilayers, all wrapped around a central rodlike micelle. Such coaxial cylinders had an overall diameter of ca. 150 nm. They were aggregated into a hexagonal-like structure.
1. INTRODUCTION The crystalline mesoporous materials designated as M41S [1] have been for the last few years the subject of increasing attention. These materials are prepared hydrothermally via a supramolecular templating technique in the presence of surfactants. Synthetic methods using anionic, cationic, gemini or neutral surfactants, under either very basic or strongly acidic conditions [2-4] were developed. Thermally stable structures, particularly the so-called MCM-41 hexagonal structure have promising applications as catalysts and as advanced materials. Potential catalytic applications of such materials were reviewed recently [5]. Early investigations focussed on silicate and aluminosilicate materials [1]. Further work dealt with the incorporation of other metal cations such as Ti [6], V [7] and B [8] into MCM-41 silicates. In addition, Huo et al. [2] first reported on open-structure networks of a number of metal oxides like W, Sb, Zn, Pb, Mg, AI, Mn, Fe, Co, Ni and Zn oxides. Most of these oxides exhibited lamellar structures, except for W (hexagonal and lamellar), Sb (hexagonal and cubic) and Pb (hexagonal and lamellar) oxides. None of these oxide mesophases including the hexagonal phases was stable upon calcination. More recently, we were able to synthesize lamellar and hexagonal ZrO2
38 [9] and to stabilize the hexagonal phase [10]. Stable hexagonally packed mesoporous titania was also synthesized [11]. Abe et al. [12] prepared hexagonal vanadiumphosphorus oxides, but no information regarding their thermal stability was provided. Aluminophosphates (AIPO4) are crystalline microporous materials prepared hydrothermally, mostly in the presence of amine templates [13]. Several AIPO4s were also prepared using linear alkylene diamines [14] or cyclic diamines [15]. Recently, we extended the so-called liquid crystal templating mechanism to the synthesis of lamellar AIPO4s with d-spacings in the nanometer range [16,17]. Lamellar AIPO4s prepared in the presence of surfactants were also the subject of two other reports [18,19]. In this paper we present an overview of our findings with particular emphasis on samples prepared with the following gel composition P2Os : 0-2 AI203 : C~2H2sNH2 : 60 H20. 2. E X P E R I M E N T A L
Several series of AIPO 4 materials were prepared hydrothermally using the gel composition: x P205 : Y AI208 : z R-NR' 2 : w H20, where x = 1.0 (or 0 for P free samples), y = 0 to 2.0, z = 0.125 to 2.0 and w = 60 to 300. The template R-NR' 2 was a primary (R' = H) or a tertiary (R'= CHs) amine with a long alkyl chain (R = CnH2n§ with n = 8 to 16). However most samples were prepared in the presence of dodecylamine. These samples will be referred to as AIPO4-x:y:z:w. The following is a typical synthesis procedure of a AIPO4 sample with a molar gel composition: P2Os : AI203 : C~2H25NH2 : 60 H20. A suspension of 2.42 g of alumina (72 % pseudoboehmite alumina, Catapal B from Vista) in 5 g of water was mixed with 4 g of phosphoric acid (Fisher Scientific, 85 %) diluted with 13 g of water and stirred for about 1 h. Finally 3.2 g of dodecylamine surfactant was added to this mixture and stirred for one additional hour. The gel was then heated under autogenous pressure at 100 ~ for 24 h in a Teflon lined autoclave with no stirring. X-ray diffraction measurements were carried out on a D5000 Siemens diffractometer (CuKec radiation, ~, = 0.15418 nm). Transmission electron micrographs were obtained as reported elsewhere using a Philips CM20 instrument operated at 200 kV [17,20]. Thermogravimetric measurements were performed on a Mettler TG50 thermobalance in a flow of air. The temperature was raised at a rate of 10 ~ up to 600 ~ s~p and 27AI MAS NMR spectra were obtained on a Bruker AMX-300 (magnetic field 7.05 T, Larmor frequencies 78.18 and 121.47 MHz, respectively) and a Bruker AMX600 (magnetic field 14.1 T, Larmor frequencies 156.36 and 242.95 MHz) spectrometers. Typical MAS speeds of rotation were 10-14 kHz, and the delay times were set at 60 s for 3~p and 0.3 s for 27A1. A conventional one-pulse sequence in combination with high power proton decoupling (40 kHz) was used for both nuclei. Very short radiofrequency pulses were employed for 27AI (0.6 l~S) in order to obtain spectra for quantitative measurements [21]. A 5 mm High Speed Probe and a 5 mm Ultrasonic Speed Probe, both from DOTY Scientific were used on the AMX-300 and AMX-600, respectively. 85% H3PO4 and a 1 M solution of aluminum nitrate were used as external references. All values for the 27AI chemical shifts reported here were corrected for the second order quadrupolar interactions [22].
39 ~3C and ~SN CP MAS spectra were collected on a Bruker AMX-300 spectrometer (Larmor frequencies 75.5 and 30.1 MHz, respectively). The speed of rotation was within 3-3.5 kHz, and the CP contact time was 2 and 5 ms for ~3C and ~SN, respectively. Signals from tetramethylsilane (TMS) and the NO3" group of solid NH4NO3 were used as external references. 3. RESULTS AND DISCUSSION
Tanev et al. [6a] were the first to use long chain primary amines as supramolecular templates for the synthesis of pure and Ti-modified hexagonal mesoporous silicates. The same technique was extended to V-modified silicates [7] and to aluminophosphates [16,17]. Recently, Oliver et al. [19] prepared lamellar AIPO4s using decylamine in a non-aqueous tetraethylene glycol solvent. In the present study both primary and tertiary amines were used. ~SN and ~3C CP MAS NMR showed that amines occluded in the as-synthesized materials were actually protonated. The ~SN signal shifted from -346.0 ppm for pure dodecylamine to -340.0 + 0.4 ppm for the occluded molecule. Likewise, the ~3C chemical shift was 43.1 and 40.2 + 0.4 ppm for pure and occluded dodecylamine, respectively. The magnitude of these shifts corresponds to protonation. The effects of AI2OJP205, C~2H2s-NH2/P2Osand H20/P205 ratios as well as the effect of the alkylamine chain length were investigated systematically. All our AIPO4 materials had lamellar structures, and consequently collapsed upon high temperature calcination. The lamellar nature of these phases was inferred from the presence of only ( 001 ) XRD peaks, and also from direct TEM observations. Figure 1 shows a series of XRD patterns for AIPO4-1:y:1:60, with y = 0 to 1.8. Samples with low AI content (y = 0 to 0.4) exhibited a lamellar phase with doo~ = ca. 22.5 A. As seen below, 8~p NMR data of these samples are consistent with the occurrence of dodecylammonium dihydrogen phosphate. Recently, Oliver et al. [20] used a similar procedure to synthesize decylammonium dihydrogen phosphate. Gels with A I / P ratios higher than 0.6 gave a lamellar AIPO4 phase with doo~= 32.5 + 0.5 ,~ (Table 1). Figure 2, a representative micrograph of AIPO4-1:1:1:60, shows alternating dark and light fringes, indicative of the occurrence of layers viewed edge-on. The electron diffraction pattern is also consistent with the presence of a layered structure with a primary repeat distance of 31 A, in good agreement with XRD measurements. In addition, as shown in Figure 3, some samples exhibited extended areas with unique structural features. These areas consist of disks with an overall diameter of ca. 150 nm aggregated into a hexagonal-like army. A close-up (Figure 4) shows that each disk is comprised of alternating dark and bright concentric rings. The primary distance between dark rings was 31 A, indicating that this new mesophase is related to the layered structure shown in Figure 2. The central tubule of the disk had a diameter of ca. 36 A, consistent with the presence of a surfactant rodlike micelle. The concentric growth of rings to form self-organized, large disks with comparable diameters was interpreted as follows [17]. Because of their small head, long chain alkylammonium surfactants tend to self-organize into planar bilayers [23]. Consequently, in the presence of inorganic species, the formation of lamellar structures is strongly favored.
40
y=1.8 1.6
1.2 1.0
5
: ".';-:,.':~Y.. ~:.'Y/',,d,~ c ?;,.-x./lx.,r, fl.fJ'~ 9 . ..... ;11 ~
",<.x.,, :,.
0.8 k0.6 k.
jk o.o '
1.5
I
'
I
,
I
3.5 5.5 7.5 2 Theta (degrees)
,
I
9.5
Figure 1: XRD pattems of AIPO4-1:y:1:60 samples. Values of y are shown on the right-hand side.
Figure 2: TEM image and its corresponding selected area electron diffraction (Ref. 17).
Table 1 Properties of AIPO4-1:y:1:60 samples. l
AI/P (y)
doo1 (A)
31p ppm
27AI (Td) ppm
0 0.2
0.8 1.0 1.2 1.4 1.6 1.8 2.0 oo
32.5 32.5 33.2 32.7 32.2 32.2 32.7 am c
0.6; 2.3 s 1.0 s; -19.3 s 1.0 s; -19.0 s 0.65 s; 2.26 s -18.6 s; -19.1 s -23.8 s; -25.8 s -13.0 b -13.0 b -13.0 b -13.0 b -13.0 b -3.8 s; -13.0 b -3.0 s; -13.0 b .
-
0.6
22.3 22.6 22.6 29.7
0.4
27AI (Oh) ppm
-
-
47.4 sm 44.5 sm 47.7 m,b 46.8 m,b 46.5 m,b 47.5 sm,b 46.8 sm,b 46.8 sm,b 46.3 sm,b .
-9.8
sh
-
-9.9 sh
-
-10.2
m,sh 10.4 s,sh 10.5 s,sh 10.4s,sh 10.7s,sh 10.4s,sh 10.0s,sh 10.3 s,sh
10.4
27AI (Oh) ppm
s
-8.5 s,b -8.7 s,b -8.5 m,b -8.0 sm,b -6.8 sm,b -6.6 sm,b -6.5sm,b
(a) bulk composition; (b) framework composition; (c) amorphous. b: broad; m, medium; s: strong; sh: sharp; sm: small.
P" AI"
-
P" A!b
-
1:0.54
-
-
-
1:0.92 1:0.80 1:1.05 1:0.79 1:1.26 1:0.84 1:1.47 1:0.90 1:1.69 1:0.95 1:1.84 1:0.89 1:2.11 1:1.07
41
Figure 4: Close-up image showing altemating dark and bright concentric rings.
Fig re 3: TEM image showing disks of coP, :entdc rings packed into a he" tgonal-like array (Ref. 17).
y
1.0
20
(x = 0)
0
-20
y =2.0
D
-40 ~,.-,~
Jl\
2.0 1.8 1.6 D
1.2
(~k.~
~.o
/
_ o~
J~JL
0.6
m
r--
20(:
__>.~
9 ,~
_
0.4
0.4
0.2
0.2
0.0
'
~o
'
~
"
-1;~o"
Chemical Shift, ppm
Fig re 5.27AI MAS-NMR spectra of AIF ~)4-1:y:1:60. Values of y are shown on he left-hand side.
"2()0
100
'
510
Chemical Shift, ppm
Figure 6. 3~p MAS-NMR spectra of AIPO4-1 :y:1:60. Values of y are shown on the left-hand side.
42 However, in the present system, the occurrence of concentric growth suggests that the system has a tendency to form some rodlike micelles, but not enough to selfaggregate, for example into a hexagonal structure. These rodlike micelles play the role of nuclei for further concentric growth of alternating rings of inorganic AIPO4 materials (dark rings) and cylindrical vesicles of surfactant (bright rings). This unique morphology is to be regarded as an example of the occurrence of new surfactantinorganic mesophases which have no lyotropic surfactant liquid crystal counterparts. Using gemini surfactants, Huo et al. [24] also discovered a surfactant-silicate mesophase with three dimensional hexagonal symmetry which has no analog among known surfactant liquid crystal structures. Likewise, Oliver et al. [19] while studying the synthesis of lamellar aluminophosphates in the presence of decylamine in a nonaqueous tetraethylene glycol solvent, found that parts of their samples exhibit remarkable morphologies and surface patterns akin to the naturally occurring silicious skeletons of diatoms and radiolaria. Figures 5 and 6 show the 27AI and 31p NMR spectra of AIPO4-1:y:1:60 samples. Detailed data are given in Table 1. Figure 5 shows that most samples exhibit three different 27AI NMR signals. Based on literature data [25], the signal at ca. 47 ppm was assigned to tetrahedral aluminum (species A) bonded to four P atoms via oxygen bridges. In agreement with Rocha et al. [27] who found that 27AI in AI(OP)4(OH2)2 resonates between -9.5 and -12 ppm, the peak at -6 to -10 ppm was attributed to framework octahedral aluminum (species B) coordinated with water and PO4 groups. Samples with low AI content (y = 0.2 and y = 0.4) exhibited only one sharp 27AI NMR peak at ca. -10 ppm corresponding to the hydrated six-coordinated AI in AIPO4 framework. Upon vacuum treatment of the samples at room temperature, the peak of species A decreased in favor of species B. This indicates that (i) both species are related to each other, and (ii) species B is coordinated to at least two water molecules. At higher AI loading (y > 0.8) a third signal with a chemical shift of ca. 10.3 ppm developed. As seen, the amorphous P free sample exhibits only one 27AI NMR signal at 10.3 ppm. It is therefore inferred that the 10.3 ppm peak observed for AI rich samples corresponds to extraframework alumina. Figure 6 shows the 31p MAS-NMR spectra of the same AIPO4-1:y:1-60 series of samples. The aluminum free sample exhibited two 3~p NMR signals at 2.3 (40 %) and 0.6 (60 %) ppm. The anisotropy (AS = -75 + 5) and the asymmetry parameter (11 = 0.3 __. 0.1) were very similar for both species. These parameters, common for acid ammonium phosphates, were assigned to two non equivalent PO2(OH)2 anions belonging to dodecylammonium dihydrogen phosphate. Samples with AI to P ratios in the range 0.8 to 1.6 exhibited a broad 3~p NMR peak centered at -13 ppm, thus excluding the presence of P sites with P in their second coordination shells. This peak was attributed to tetrahedral P bonded to (4 - X) aluminum tetrahedra and X hydroxyl groups (where X = 1 or 2). The chemical shifts of 3~p in microporous AIPO4s generally fall in the range of -19 to -30 ppm [27]. The downfield shift observed for our samples may due to several factors, particularly for the hydrophillic nature of the materials [28]. The origin of the peak broadening is most likely attributable to the occurrence of a distribution of P sites with similar but not identical environments. This conclusion stems from the fact that at higher field (14.1 T) the resolution of the peak hardly improved. The first derivative of the 31p NMR signal
43 indicates the presence of at least five subgroups of P sites (Figure 6, inset). In addition to the -13 ppm 31p signal, samples with the highest levels of AI displayed a low intensity (< 4%), sharp peak at ca. -3.4 ppm attributed to an impurity phase. For samples with very low AI contents (y = 0.2 and y = 0.4) there was a sharp peak at -19 ppm in addition to the Sip peak close to 0 ppm observed in the AI-free sample. This -19 ppm 31p peak together with the -10 ppm 27A! peak observed for the same sample may correspond to variscite: AIPO4-2H20 with 5(~IP) = -19.5 ppm and ~(27AI) = -11 ppm [29]. If this assignment is correct, the variscite phase must be highly dispersed not to be observed by XRD. As seen in Table 1 (column 7), the overall AI/P ratios of the samples are comparable to those of the corresponding gels. The framework P to AI ratios shown in the last column represent ratios of the sum of AI species A and B to P calculated based on chemical analysis, quantitative AI NMR data and assuming complete retention of phosphorus. It is seen that AI/P is usually below one. As inferred from NMR data, this indicates the occurrence of some P-O +NH3-C12H2slinkages. Additional data on the effect of other synthesis parameters will be published elsewhere [30].
4. CONCLUSIONS A variety of lamellar aluminophosphates with doo~distances in the range of 2-4 nm were synthesized via the supramolecular templating mechanism using long chain primary and tertiary alkylamines as templates. The effects of other synthesis parameters were also studied. The occurrence of lamellar phases was inferred from XRD data and by direct TEM observations. 81p and 27AIdata were consistent with the presence of aluminophosphate. Even though the synthesis variables had strong effect on the quality of the products formed and on the connectivities of AI and P, they did not favor the formation of three dimensional AIPO4 structures. In addition to the main phase with planar lamellae, some samples exhibited extended areas consisting of coaxial cylinders of altemating inorganic aluminophosphate material and organic surfactant bilayers, all wrapped around a central rodlike micelle. Such coaxial cylinders which were aggregated into a hexagonal-like structure had an overall diameter of ca. 150 nm.
Acknowledgments Partial funding by the Natural Sciences and Engineering Research Council (NSERC) of Canada is acknowledged. I wish to thank I.L. Moudrakovski, J.S. Reddy, V.R. Karra, C.I. Ratcliffe, J.A. Ripmeester, K.F. Preston, A. Chenite and Y. Le Page for significant contributions to this work.
REFERENCES (a) C.T. Kresge, M.E. Leonowicz, J.C. Vartuli and J.S. Beck, Nature, 359 (1992) 710.
44
.
=
4. 5. 6.
.
.
.
10. 11. 12. 13. 14.
15. 16. 17. 18.
19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30.
Q. Huo, D.I. Ciesla, D.G. Demuth, P. Feng, T.E. Gier, P. Sieger, A. Firouzi, B. Chmelka, F. Sch0th and G.D. Stucky, Chem. Mater., 6 (1994) 1176. P.T. Tanev and T.J. Pinnavaia, Science, 267 (1995) 865. S.A. Bagshaw, E. Prouzet and T.J. Pinnavaia, Science, 269 (1995) 1242. A. Sayari, Chem. Mater. (1995), submitted for publication. (a) P.T. Tanev, M. Chibwe and T.J. Pinnavaia, Nature, 368 (1994) 321. (b) A. Corma, M.T. Navarro and J. Perez-Pariente, J. Chem. Soc., Chem. Commun., (1994) 147. (c) A. Sayari, V.R. Karra and J.S. Reddy, Mat. Res. Soc. Symp. Proc., 371 (1995) 87. (a) K.M. Reddy, I.L. Moudrakovski and A. Sayari, J. Chem. Soc., Chem. Commun., (1994) 1059. (b) J.S. Reddy and A. Sayari, J. Chem. Soc., Chem. Commun., (1995) 2231. (d) J.S. Reddy and A. Sayari, Appl. Catal., (1995), submitted for publication. (a) A. Sayari, C. Danumah and I.L. Moudrakovski, Chem. Mater., 7 (1995) 813. (b) A. Sayari, I.L. Moudrakovski, C. Danumah, J.A. Ripmeester, C. Ratcliffe, C. and K.F. Preston, J. Phys. Chem., 99 (1995) 16373. J.S. Reddy and A. Sayari, Catal. Lett., (1996), in press. J.S. Reddy, P. Liu and A. Sayari, 1996 Spring Meeting of the Materials Research Society, San Diego, (1996). D.M. Antonelli and J.Y. Ying, Angew. Chem. Int. Ed. Engl., 34 (1995) 2014. T. Abe, A. Taguchi and Iwamoto, Chem. Mater., 7 (1995) 1429. (a) S.T. Wilson, B. Lok, C.A. Messina, T.R. Connan and E.M. Flanigen, J. Am. Chem. Soc., 104 (1982) 1146. (b) S.T. Wilson, Stud. Surf. Sci. Catal., 58 (1991) 137. (a) R.H. Jones, A.M. Chippindale, S. Natarajan and J.M. Thomas, J. Chem. Soc., Chem. Commun., (1994) 565, and references therein. (b) B. Kraushaar-Czametzki, W.H.J. Stork and R.J. Dogterom, Inorg. Chem., 32 (1993) 5029. P.A. Barrett and R.H. Jones, J. Chem. Soc., Chem. Commun., (1995) 1979. A. Sayari, V.R. Karra, J.S. Reddy and I.L. Moudrakovski, J. Chem. Soc., Chem. Commun., (1996), in press. A. Chenite, Y. Le Page, V.R. Karra and A. Sayari, J. Chem. Soc., Chem. Commun., (1996), in press. C.A. Fyfe, W. Achwieger, G. Fu and G.T. Kokotailo, Prepr., A.C.S. Div. Petrol. Chem., 40 (1995) 266. S. Oliver, A. Kuperman, N. Coombs, A. Lough and G. Ozin, Nature, 378 (1995) 47. A. Chenite, Y. Le Page, Y. and A. Sayari, Chem. Mater., 7 (1995) 1015. P.P. Mann, J. Klinowski, A. Trokiner, H. Zanni and P. Papon, Chem. Phys. Left., 151 (1988) 143. G. Engelhardt and D. Michel, High-Resolution Solid-State NMR of Silicates and Zeolites, Wiley, Chichester, 1987. J.N. Israelachvili, Intermolecular and Surface Forces, Academic Press, NY, 1991. Q. Huo, R. Leon, P.M. Petroff and G.D. Stucky, Science, 268 (1995) 1324. D. Muller, E. Jahn, G. Ladwig, G. and V. Haubenreisser, Chem. Phys. Lett., 109 (1984) 332. J. Rocha, W. Kolodziejski, H. He and J. Klinowski, J. Am. Chem. Soc., 114 (1992) 4884. I.L. Moudrakovski, V.P. Schmachlova, N.S. Katsarenko and V.M. Mastikhin, J. Phys. Chem. Solids, 47 (1987) 335. L.S. de Saldarriaga, C. Saldarriaga and M.E. Davis, J. Am. Chem. Soc., 109 (1987) 2686. C.S. Blackwell and R.L. Patton, J. Phys. Chem., 92 (1988) 3965. A. Sayari et al., Chem. Mater. (1996), submitted for publication.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
45
Synthesis and Hydrothermal Stability of a Disordered Mesoporous Molecular Sieve Ryong R y o o a, J. M. Kim', C. H. Shinb and J. Y. Lee c
"Departmem of Chemistry, KAIST, Taejon, 305-701, Korea; bCatalysis Research Division, KRICT, Taejon, 305-606, Korea; CDepartment of Materials Science and Engineering, KAIST
A noncrystalline mesoporous molecular sieve has been synthesized by hydrothermal polymerization of silicate and aluminate anions surrounding the molecular organization of hexadecyltrimethylammonium chloride in the presence of various organic polyacids. The noncrystalline molecular sieve is very similar to the well-known mesoporous molecular sieve MCM-41 in the aspect of the high specific surface area and uniform pore sizes, but the channel arrangement interconnected in a three dimensional disordered way distinguishes it most conspicuously from the MCM-41 which exhibits hexagonal arrangement of straight channels. The disordered structure has remarkably high hydrothermal stability and thermal stability, compared with MCM-41 and MCM-48.
1. Introduction In recent years, there have been dramatic advances in the concept of molecular sieves exhibiting uniform pore sizes. The structures of early molecular sieves were typified by crystalline microporous materials such as zeolites and AIPO4 in which the arrangement of channels (or pores) and the arrangement of framework atoms are ordered over crystallographically long range. Later, the discovery of crystalline mesoporous molecular sieves such as MCM-41 and MCM-4813 has opened a new class of molecular sieves in which only the channel arrangement is crystallographically ordered while the atomic arrangement is disordered similar to amorphous silica. Since then, a few silicate materials exhibiting disordered arrangement of mesopores with very high specific surface areas of approximately 1000 m2g1 began to attract our attention. One such material was synthesized by Chela et al. 4 using hydrothermal reaction of Na-kanemite and hexadecyltrimethylammonium (HTA) chloride. The material gave a N2 adsorption isotherm similar to that for MCM-41, which indicated that the pore size distribution was similar to that for the MCM-41. The structure of the material was illustrated by the authors with straight mesoporous channels which were entangled randomly. Bagshaw et al. s obtained another disordered mesoporous material designated MSU=I using tetraethylorthosilicate and nonionic surfactants. Guo 6 also reported a similar material. The pore size distribution curves for these two mesoporous silicate materials showed peak widths greater than 0.9 nm, which was about three times broader at the
46 half height than that for MCM-41. Although the pore structures of the materials were still very heterogeneous compared with the pore sizes for the crystalline MCM-41 and MCM-48, their discovery showed a possibility of finding noncrystalline molecular sieves with uniform pore sizes. Very recently, efforts to obtain such noncrystalline molecular sieves with truly uniform pore sizes have succeeded by the present authors using hydrothermal polymerization of silicate and aluminate anions surrounding the molecular organization of hexadecyltfimethylammonium chloride in the presence of various organic polyacids. 7 The disordered molecular sieve thus obtained is very similar to the MCM-41 in the aspect of the high specific surface area and uniform pore sizes, but the channel arrangement interconnected in a three dimensional disordered way distinguishes it most conspicuously from the MCM-41 which exhibits a hexagonal arrangement of straight channels. Besides, the disordered structure has higher thermal stability and hydrothermal stability than MCM-41 structure. Here, we describe details of the synthesis method and the hydrothermal stability of the disordered mesoporous molecular sieve exhibiting uniform pore sizes.
2. Experimental A fully disordered surfactant-silicate mesostructure has been obtained using sodium silicate, alkyltrimethylammonium (ATA) halide (CnHz~+IN(CH3)3X, n = 12 - 18, and X = Cl or Br) and sodium salt of organic polyacid. Typical procedures to obtain the disordered mesostructure were as follows: a clear solution of sodium silicate with a Na/Si ratio of 0.5 was first prepared by combining 46.9 g of 1.00 M aqueous NaOH solution with 14.3 g of a colloidal silica, Ludox HS40 (39.5 wt% SiO2, 0.4 wt% Na20 and 60.1 wt% H20, Du Pont) and heating the resulting gel mixture with stirring for 2 h at 353 K. The sodium silicate solution was dropwise added to a polypropylene bottle containing a mixture of 0.29 g of 28 wt% aqueous NH3 solution, 23.8 g of ethylenediaminetetraacetic acid tetrasodium salt (Na4EDTA), 20.0 g of 25 wt% HTACI solution and 28.0 g of doubly distilled water, with vigorous magnetical stirring at room temperature. The resulting gel mixture in the bottle had a molar composition of 4 SiO2 91 HTACI : 4 Na4EDTA : 1 Na20 : 0.15 (NH4)20 : 350 H20. After stirring for 1 h more, the gel mixture was heated to 370 K for 2 d. The resulting mixture was cooled to room temperature. Subsequently, pH of the mixture was adjusted to 10.2 by dropwise addition of 30 wt% acetic acid with vigorous stirring. The reaction mixture after the pH adjustment was heated again to 370 K for 2 d. This procedure for pH adjustment to 10.2 and subsequent heating for 2 d was repeated twice more. The precipitated product was filtered, washed with doubly distilled water and dried in an oven at 370 K. The product was calcined in air under static conditions using a muffle furnace. The calcination temperature was increased from room temperature to 823 K over 10 h and maintained at 823 K for 4 h. The calcined product is designated KIT-1. The product yield was more than 90%, based on the silica recovery. Aluminum-containing KIT-1 (AIKIT-l) samples with Si/Al as high as 5 have been obtained by adding 5 wt% aqueous solution of sodium aluminate (Strem, 99.9% on metal basis) during the formation of the above disordered surfactant-silicate mesostructure. The aluminate solution was added to the reaction mixture at room temperature following the second heating
47 step to 370 K, dropwise with vigorous mixing. The second pH adjustment o f the reaction mixture with acetic acid was carried out after the resulting surfactant-aluminosilicate gel mixture was heated for 2 d. The remainder of the synthesis procedure was the same as the preparation of the above pure silica K/T-1. Hydrothermal stability of the samples was investigated by measuring the intensity decrease in powder X-ray diffraction (XRD) pattern during heating in doubly distilled water. The sample to water ratio was fixed as 1 g.L q. Samples at~er the heating in water were filtered, washed in doubly distilled water, and immediately placed in oven to dry for 2 h at 400 K. XRD patterns were obtained from the samples with a Cu K~ X-ray source using a Rigaku D/MAXIII (3 kW) instrument.
3. Results and Discussion
Characterization of a disordered molecular sieve. Figure 1 shows XRD patterns for the disordered HTA-silicate mesostructure obtained using Na4EDTA The surfactant is easily
5
3
m
m
|
m
20
I
I
2
4
I
6 Two theta
!
8
10
Figure 1. Powder X-ray diffraction patterns for a fully disordered molecular sieve, KIT-l, synthesized using HTAC1 as a template. Inset, the relationship between dl0o spacing and number of carbon atoms in the surfactant chain: (0) as-synthesized and (r-l) calcined.
48 removed from the mesostructure by calcination in air under static conditions at any temperatures between 823 - 1173 K. Strict conditions using gas flows are not required for the calcination. Both the as-synthesized product and the calcined material exhibit same XRD patterns with three broad peaks indexed to (100), (200) and (300) diffraction with dl00 = 4.0 4.2 nm. The XRD intensity increases approximately 3 times upon calcination due to the removal of the surfactant. The dl00 spacing decreases very slightly (___0.1 nm) upon the calcination. The three-line XRD pattern is similar to the XRD pattern for a layered material. But, the KIT-1 is not a layered material since the removal of the surfactant by the hightemperature calcination does not lead to the structure collapse. The pore size distribution for the calcined KIT-1 material has been obtained from N2 adsorption-desorption isotherms at liquid N2 temperature following the Horvath-Kawazoe analysis, s The pore-size distribution curve in Figure 2 shows a mesopore with the pore diameter 3.4 nm at maximum of the distribution. The specific surface area for the KIT-1 has been obtained to be 1000 megq by the BET method, which is similar to MCM-41. It is remarkable that the mesopore structure of the KIT-1 (~ 0.3 nm peak width) is as uniform in pore size as the crystalline MCM-41 (~ 0.3 nm peak width) la on the basis of the width at half maximum for the pore size distribution curve. Thus, the individual pore widths are truly uniform inside the disordered structure of the KIT- 1.
-
~, 700 ~
600-
500 400 300 200 lO0 0 0
0.2
0.4
0.6
0.8
1.0
Relative pressure (P/P0)
I
I
I
I
I
I
I
I
I
I
1
2
3
4
5
6
7
8
9
10
Effective pore size (nm) Figure 2. Pore size distribution curve obtained by the Horvath-Kawazoe analysis for a disordered molecular sieve, KIT-I, alter calcination. Inset, the corresponding N2 adsorption-desorption isotherms.
49 As shown by a transmission electron micrograph (TEM) in Figure 3, the disordered surfactant-silicate mesostructure is similar to a bicontinuous structure arranged in a threedimensional disordered way. The calcined product KIT-1 also gives essentially the same transmission electron micrograph as the as-synthesized form. No long range structural order has been found from the electron diffraction pattern. Compared with the hexagonal structure of MCM-41, it is believed that the organic polyacids anions causes fluctuation in the surfactant micellar arrangement, giving rise to the formation of a stable isotropic labyrinth or disordered sponge phase that is similar to the so called L3 phases known in surfactant solutions. 9 However, the arrangement of the mesoporous channels in the KIT-1 structure is distinguished from the L3 phase by the intercormection of the mesoporous channels by numerous branches.
30nm
Figure 3. Typical transmission electron micrograph: (a) MCM-41 and Co) fully disordered molecular sieve, KIT-1. We have performed the following two experiments in order to investigate if the structure of the KIT-1 consists of one-dimensional mesoporous channels entangled in a disordered way, or the structure has very short channels interconnected by numerous branches. In one of the experiments, aluminum has been incorporated within the KIT-1 framework over the range of Si/AI = 5 - oo using sodium aluminate during synthesis, and the experimental conditions for the removal of surfactant by calcination have been compared with those for AIMCM-41. Our results show that the synthesis of AIMCM-41 leads to progressive decreases in the XRD intensity and increases in the line width, due to losses in the structural order as the AI content ihcreases beyond 15 Si/A1.~~ Moreover, calcination of the as-synthesized products with high AI content leads to the formation of coke due to the surfactant decomposition, which causes
50 channel blockage. The coke formation can be prevented by washing a large fraction of the surfactant using an ethanol-HCl mixture prior to the calcination. However, significant dealumination occurs during the washing. The resulting A1MCM-41 gives low ion exchange capacity, and furthermore much of the structural order is lost during the cation exchange due to weak hydrothermal stability of the MCM-41 samples, a~ Compared with the AIMCM-41, calcination of the AIKIT-1 can be performed using air under static conditions without washing with the ethanol-HCl mixture, which is indicative of facile diffusion of gases through numerous branches in the three dimensional channel structure during calcination. In the second experiment, Pt clusters about 3 - 4 nm in diameter have been supported inside the mesoporous channels of MCM-41 and KIT-1 following an impregnation technique using HzPtCI6. Catalytic activity of the Pt-supporting samples for hydrogenolysis of ethane with 1-12 has been measured using a batch recirculation reactor. The Pt clusters are large enough to cause multiple pore blockage in the MCM-41 channels, and thus the surface atoms on the Pt clusters located inside the one dimensional channel of the MCM-41 are not accessible for the catalytic hydrogenation, n On the other hand, the Pt clusters supported inside the three dimensional channel structure of the KIT-1 are fully accessible for ethane hydrogenolysis with H2. Thus, the catalytic activity for the Pt/KIT-1 is proportional to the Pt loading. It is clear that the presence of the three-line XRD pattern for the KIT-1 comes from a short range structural order with very uniform pore sizes. Similar products can be obtained if the Na4EDTA is substituted by sodium salts of adipic acid, other polycarboxylic acids and polysulfonic acids. The products obtained with different polyacids give similar XRD patterns with three broad diffraction bands. The line widths and line shapes can be somewhat dependent on the different polyacids and also on the salt concentration. This is probably due to differences in the density of the branches interconnecting the channels and the distance between adjacent branches, which determine the local structure of the KIT-1. It is believed that the channel disorder in the KIT-1 structure can be controlled by the nature and concentration of the chemical agents used to induce the fluctuation in the micelle arrangement. Likewise to the MCM-41,1'2 it is also possible to tailor the channel widths by use of surfactants with suitable sizes. The dl00 spacings for the calcined materials are plotted against the number of carbon atoms in the ATA surfactant in Figure 1.
Hydrothermal stability of mesoporous molecular sieves. MCM-411a and other mesoporous molecular sievess'6,a3 found recently have opened new possibilities as a support for adsorption and catalysis, and also as a template for architecting nanosize materials. The mesoporous material, MCM-41 has excellent thermal stability up to 1170 K or higher in air and 02. The stability is not affected considerably by the presence of' water vapor up to 2.3 kPa in the 02 flow. 14'as Furthermore, there is a report that the MCM-41 constructed with silica framework can be stable even in a 100%-steam flow under atmospheric pressure at 820 K. t~ However, contrary to the good stability at high temperatures, the MCM-41 is reported to lose the structure easily during storage in humid air and aqueous solutions at relatively low temperatures around 370 K. 11 The loss of the structure involves silicate hydrolysis as shown by Kim and Ryoo using XRD and magic angle spinning 29Si ~ spectroscopy, at The loss of the structure makes it difficult to obtain high levels of ion exchange with MCM-41. as In
51 addition, although MCM-41 has been reported to be useful for many catalytic applications, l~qs it is expected that the loss of the structure can lead to a rapid decrease in the catalytic activities with time under experimental conditions containing water or saturated with water vapor. Thus, the poor hydrothermal stability of the MCM-41 in water can be a critical problem limiting the applications. Therefore, improvement of hydrothermal stability is a target for ultimate successful uses of the MCM-41 type materials. We have obtained pure silica MCM-41 and MCM-48 samples, following hydrothermal synthesis procedures reported in the literature, 1-3 and compared hydrothermal stability of the
KIT-1
MCM-48
MCM-41
C
~
C
b ~~_______
b
!
2
4
6
8
Two theta
2
4
6
8
Two theta
i
i
i
i
2
4
6
8
10
Two theta
Figure 4. Powder X-ray diffraction patterns for two crystalline mesoporous molecular sieves, MCM-41 and MCM-48, and a fully disordered molecular sieve, KIT-l, exhibiting the transmission electron micrograph in Figure 3: (a) calcined samples, (b) heated in water at 343 K for 12 h, (c) heated in boiling water for 12 h, and (d) heated in boiling water for 48 h. samples in boiling water with that of KIT-1. Figure 4 displays XRD patterns for the mesoporous materials against heating temperatures in water. The XRD patterns for the calcined MCM-41 samples before the heating in water show four dif~action lines characteristic of the hexagonal structure of the MCM-41. The XRD pattern for the MCM-48 sample agrees with the cubic 1,3d structure known in the literature. 13 No distinct changes in the structures are indicated by the XRD lines during 12 h in distilled water at room temperature. As the water temperature increases to 343 K, the intensity of the XRD patterns decreases conspicuously. Moreover, the decrease in the XRD intensity depends considerably on details of the synthesis procedures. 11 The stability difference is consistent with previous conclusion lsa9 that the stability of MCM-41 can be enhanced by repeating pH adjustment to around 11 during hydrothermal synthesis, due to an equilibrium shift of the synthesis reaction
52 condensation. 16~~ However, all the structures disappeared completely during the heating at 373 K. Compared with the weak hydrothermal stability of the MCM-41 and MCM-48 samples as shown in Figure 4, it is remarkable that the structure of the KIT-1 is stable in boiling water for 48 h. We have confirmed that the structure of the KIT-1 does not change under 100%-steam flow for 2 h at 1020 K. The disordered structure is also stable during heating with air flow containing 2.3 kPa water vapor for 2 h at 1220 K. In summary, the disordered mesoporous material, KIT-l, found in the present work belongs to a new class of molecular sieve in which the channels are interconnected in a three dimensional, fully disordered way. The structure of the material corresponds to a disordered bicontinuous phases known in surfactant solutions, in contrast to the hexagonal structure of MCM-41. Since the disordered structure, compared with the ordered MCM-41, has remarkable advantages due to the three dimensional diffusion and high hydrothermal stability, our findings of the new class of molecular sieves are expected to provide new opportunities for rational design of heterogeneous catalysts, adsorbents and other related materials requiring the three dimensional pore structure. References
1. C.T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli and J. S. Beck, Nature, 359 (1992) 710. J.S. Beck, J. C. Vartuli, W. J. Roth, M. El Leonowicz, C. T. Kresge, K. D. Schmitt, C. T.-W. Chu, D. H. Olson, E. W. Sheppard, S. B. McCullen, J. B. Higgins and J. L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. 2. A. Monnier, F. Schi~th, Q. Huo, D. Kumar, D. Margolese, R. S. Maxwell, G. D. Stucky, M. Krishnamurty, P. Petroff, A. Firouzi, M. Janicke and B. F. Chmelka, Science, 261 (1993) 1299. 3. Q. Huo, R. Leon, P. M. Petroffand G. D. Stucky, Science, 268 (1995) 1324. 4. C.-Y. Chen, S.-Q. Xiao and M. E. Davis, Microporous Materials, 4 (1995) 1. 5. S.A. Bagshaw, E. Prouzet and T. J. Pinnavaia, Science, 269 (1995) 1242. 6 C.J. Guo, Stud. Surf. Sci. Catal., 97 (1995) 165. 7. R. Ryoo, J. M. Kim, C. H. Ko and C. H. Shin, J. Phys. Chem., in press. 8. R. Ryoo et al., in preparation. 9. G. Horvath and K. J. Kawazoe, J. Chem. Eng. Japan, 16 (1983) 470. 10. R. Ryoo, S. J. Cho, C. Pak and J. Y. Lee, Catal. Lett., 20 (1993) 107. R. Ryoo, S. J. Cho, C. Pak, J.-G. Kim, S.-K. Ihm and J. Y. Lee, J. Am. Chem. Soc., 114 (1992) 76. 11. D. Roux, C. Coulon and M. E. Cates, J. Phys. Chem., 96 (1992) 4174. 12. Z. Luan, H. He, W. Zhou, C.-F. Cheng and J. Klinowski, J. Chem. Soc. Faraday Trans., 91 (1995) 2955 and references on AIMCM-41 therein. 13 J. M. Kim and R. Ryoo, Bull. Korean Chem. Soc., 17 (1996) 66. 14. R. Ryoo, C. H. Ko, J. M. Kim and R. Howe, Catal. Lett., 37 (1996) 29. 15. C.-Y. Chen, H.-X. Li and M. E. Davis, Microporous Materials, 2 (1993) 17. 16. J. M. Kim, J. H. Kwak, S. Jun and R. Ryoo, J. Phys. Chem., 99 (1995) 16742. 17. E. Armengol, M. L. Carlo, A. Corma, H. Garcia and M. T. Navarro, J. Chem. Soc., Chem. Commun. (1995) 519. 18. C.-G. Wu and T. Bein, Science, 264 (1994) 1757. 19. K. R. Kloetstra and H. van Bekkum, J. Chem. Soc., Chem. Commun. (1995) 1005. 20. R. Ryoo and J. M. Kim, J. Chem. Sot., Chem. Commun. (1995) 711.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
53
Preparation of silica-pillared molecular sieves from layered silicates Soon-Yong Jeong a, Oh-Yun Kwon b, Jeong-Kwon Suh a, Hangkyo Jin a, and Jung-Min Lee a aChemical Engineering Division, Korea Research Institute of Chemical Technology, Yusung, P. O. Box 107, Taejon, Korea 305-606 bDepartment of Chemical Engineering, Yosu National Fisheries University, Yosu, Korea 550-749 Magadiite and kenyaite were hydrothermally synthesized in Teflon-sealed stainless steel autoclave. The intercalation of TEOS(tetraethylorthosilicate) into the interlayers of layered silicates was carried out by amine preintercalation, and the effects of acid and base catalysts during gelation of TEOS into interlayers were investigated. It was found that the samples silica-pillared by acid- and basecatalyzed reactions show well-ordered basal spacing and super-gallery heights. Also, they exhibit relatively narrow pore size distributions in the range of 18-40 ,A, and show high surface areas in the range of 533-845 m2/g, depending on the catalyst types. These results indicate that the variations in the conditions of gelation contribute to improvement in physical properties of silica-pillared molecular sieves. 1. INTRODUCTION Layered silicates have attracted widespread interest over the past 20 years due to their catalytic, adsorptive and ion-exchange properties [1]. Recently, several researchers have investigated the pillared reactions of layered silicates such as magadiite, and kenyaite [2-5]. Magadiite and kenyaite were primarily found by Eugster [6] in the lake beds of the lake Magadi in Kenya. Afterward, other occurrences of these have been continuously reported in various regions [7], and these materials were mostly found from sodium carbonate-rich alkaline lake waters. They also have been successfully synthesized under hydrothermal conditions [8,9]. Their basic structures are composed of duplicated SiO 2 tetrahedral sheets, and are similar to clay minerals except to be free of aluminum [10]. Silica-pillaring of magadiite was reported by a few researchers. Landis et al. [4] found that the pillaring of magadiite could be facilitated by using a preswelling step in which the interlayers are exposed to organoammonium ion or amine. The calcined sample obtained from TEOS [Si(OC2H5)4] pillaring exhibited a high surface area, 530 m2/g. Sprung et al. [5] reported that the pillared derivatives of magadiite
.54 can be obtained from the calcination of hydrolyzed phenyltrichlorosilane-magadiites. Daily and Pinnavaia [3] synthesized supergallery derivatives on the basis of Hmagadiite by gelation of TEOS with EtOH suspension. After calcining to remove organic compounds, pillared magadiite with surface areas of about 520-680 m2/g, depending on the amount of gelled TEOS, was formed. However, the pillaring of kenyaite was rarely reported. Recently, Landis et al. [4] prepared pillared derivatives on the basis of H-kenyaite by gelation of TEOS with EtOH suspension. The calcined sample exhibited a high surface area, 600 m2/g. In the sol-gel process, solvent such as EtOH is added to prevent the liquid-liquid separation during the initial stage of the hydrolysis reaction and to control the concentration of silicate species and water that influence the gelation kinetics [11]. However, the reaction of TEOS gelation by alcohol suspension occurs very slowly, and because TEOS is alcohol-soluble, it can be released outside the layered phases during gelation. Aelion et al. [12] observed that the rate of hydrolysis of TEOS was influenced by the strength and concentration of the acid and base catalysts. The fast gelation using the catalyst such as acid or base can minimize the release of TEOS from the layered phases during gelation. Generally, TEOS gelation by acidor base- catalyzed hydrolysis could diversify the interfacial properties of products and result in such products as bulk gel, film, fiber, powder, and catalyst support. In the present work, we report the effects of acid or base catalysts on the hydrolysis and condensation polymerization of intercalated TEOS in H-type layered silicates.
2. EXPERIMENTAL 2.1 Syntheses of Na-magadiite and Na-kenyaite Synthetic Na-magadiite and Na-kenyaite were prepared by the reaction of NaOH/Na2CO3-SiO2 system under hydrothermal conditions using methods analogous to those described by Fletcher and Bibby [9]. Materials used were silica gel (Wakogel Q-63) and analytical reagent grades of NaOH and Na2CO3. Namagadiite was synthesized in a stainless steel autoclave without stirring at 150~ for 72 hrs under autogenous pressure, using mole ratios of SiO2 " NaOH NaCO3 9 H20 9 = 15 19 29 300. 9 Na-kenyaite was synthesized at 150-160 ~ for 70-80 hrs under autogenous pressure, using mole ratios of SiO2 NaOH 9 Na2CO3 9 H20 9 = 9 19 29 9 600. The products were filtered, and washed with deionized water in order to remove excess NaOH or Na2CO3, and dried at 40~ 2.2 Preparation of silica-intercalated layered silicates H-magadiite and H-kenyaite was prepared by titration of Na-kenyaite with 0.1 N HCI using the method of Beneke and Lagaly [8]. A suspension of 40g of Nakenyaite per 500ml of deionized water was stirred for 1 hr. The suspension was then titrated with 0.1 N HCI to a final pH of 2.0, and then maintained at the same value for one week in a refrigerator. H-magadiite and H-kenyaite was recovered by filtering, and washing with deionized water until CI-free and then dried in air at 40 ~
55 Octylamine/octylammonium-magadiite gel was reacted for 24 hrs at room temperature by adding 5.0 g of excess octylamine to 1.0 g of air-dried H-magadiite. An organic pillar precursor 20g of TEOS, was added to octylammonium-magadiite gel and then stirred for 24 hrs at room temperature. TEOS was then absorbed into the organophilic interlayer region. The TEOS-intercalated magadiite was separated by centrifugation from the mother liquid. Also, octylamine/octylammonium-kenyaite gel was formed by allowing air-dried H-kenyaite (0.86g, 0.57 mmol) to react at room temperature with excess octylamine (2g, 15 mmol) for 48 hrs. During octylamine addition, H-kenyaite absorbs the liquid amine, immediately forming a gelatinous mixture that will not flow. Silica-intercalated derivatives of kenyaite were prepared by the reaction of excess TEOS (15g, 72 mmol) with a gel composed of octylammonium-kenyaite solvated by excess octylamine for 24 hrs at room temperature. The TEOS-intercalated product was separated by centrifugation from the mother liquid. Gelation of the intercalated TEOS without catalyst was carried out by drying EtOH (10ml) suspension of TEOS-intercalated products at 40~ in air. EtOH was mixed with 3 N NH4OH and 0.1 N HCI in order to examine the effects of base and acid catalysts during the gelation. The compositions of acid and base catalysts are shown in Table 1. Gelation was conducted with stirring for 20 min. after addition of 10 ml of each catalyst to the TEOS-intercalated magadiite and kenyaite at room temperature. The stoichiometry and methodology of gelation of TEOS are wellknown, and the physical characterization of gelled silicate has been studied by several researchers [11, 13]. The gelled samples were filtered from the mother liquid, and dried in air, and then calcined at 538~ for 4 hrs in air to remove water, intercalated organoammonium ion, and organic byproducts from TEOS hydrolysis. Basal spacings of samples were determined from the 00~ X-ray powder diffraction using a Rigaku diffractometer equipped with CuK(z radiation. Nitrogen adsorption/desorption isotherms were determined by Micromeritics ASAP 2000 at 77K. All samples were outgassed at 300~ under a vacuum for 4 hrs. Surface area was determined by the BET equation. Micropore volume was obtained from t-plot methods [14], and the pore size distributions of silica-pillared products were determined by the BJH equation [15]. Table 1 Compositions of catalysts (wt%) EtOH
H20
HCl
NH3
No catalyst
95.0
5.0
Base-catalyst
16.5
79.2
-
4.3
Acid-catalyst
64.8
35.2
0.01
-
56
3. RESULTS AND DISCUSSION 3.1 Syntheses of magadiite and kenyaite The basic hydrolysis of silica gel at 150~ according to the method of Fletcher and Bibby [9] produced well-crystallized Na-magadiite and Na-kenyaite. The X-ray powder diffraction patterns of the air-dried products, shown in Fig. l(a, c) exhibited several 00~ reflections corresponding to a basal spacing of 15.6 A for Na-magadiite and 20 A for Na-kenyaite. The peak positions for this synthetic product agree closely with values reported previously [8]. The slow titration of Na-magadiite and Na-kenyaite with 0.1 N HCI resulted in the exchange of sodium ions for protons in the layered structure. The X-ray of powder diffraction patterns of H-magadiite and H-kenyaite exhibited 00~ reflections corresponding to a basal spacing of 12.6 A for H-magadiite and 18.0 A for H-kenyaite (Fig. 1 (b, d)), in agreement with earlier work [9]. The decrease in basal spacing indicated a loss of interlayer H20 upon replacement of Na* by H*.
. =,..,
==
C
=.=.=
. =,,=,
,=..=
n,' d I
I
I
I
I
I
i
I
I
I
I
I
i
I
I
I
I'
I
I
I
I
I
5 1015202530354045505560
5 1015202530354045505560
20
20
Figure 1. X-ray diffraction patterns of (a) Na-kenyaite (b) H-kenyaite (c) Namagadiite and (d) H-magadiite.
3.2 Preparation of silica-intercalated layered silicates 3.2.1 Silica-pillared magadiite The X-ray diffraction patterns and basal spacings of the calcined silica-pillared magadiites are shown in Fig. 2 (a, b, c) and Table 2. The silica-pillared magadiites gelled by base- and acid-catalyzed reactions indicate a large increase in basal spacing of 39.2 and 33.3 A, compared with the basal spacing of EtOH gelled product (17A). Table 2 shows the physical properties of the porous silica-pillared magadiites. The surface area of the sample gelled by EtOH suspension was 587
57 m2/g, coinciding with the result of Daily and Pinnavaia [3]. The sample produced by base or acid catalyst has a higher surface area and larger total pore volume than that gelled by no catalyst. These results can be explained by the point that the hydrolytic polycondensation of intercalated TEOS by acid and base catalyst could form silica clusters of more highly branched and stiff network structure. Pillared silica clusters expand the space between layered phases and affect the development of micropocity and the increase of surface area. These effects are most evident when intercalated TEOS is not released outside the layered phase during gelation. Figure 3(a) shows that the pore size distributions of silica-pillared magadiites. The sample treated with the base-catalyzed gelation has more microposity (diameter < 20 A ) and shows a sudden increase in mesopore volume near 36 A with a narrow pore size distribution. These results indicate that abrupt gelation by base catalyst is closely related to the formation of a more uniform pore. On the other hand, the sample gelled by the suspension of EtOH has a broad pore distribution. In case of gelation by acid catalyst, microporosity decreases and mesoporosity increases between 40 and 100 A compared with gelation with no catalyst.
IN,
t~ t-'
E
i
1 e
n,,
I
2
'
1'2
Degree 2e
I
18 20
4 6 8
I()121416
1'820
Degree 20
Figure 2. X-ray diffraction patterns of the calcined silica-pillared layered silicates: (a) magadiite gelled by EtOH suspension (b) base-catalyzed magadiite (c) acidcatalyzed magadiite (d) acid-catalyzed kenyaite (e) base-catalyzed kenyaite (f) kenyaite gelled by EtOH suspension.
.58 Table 2 Physical properties of silica-pillared magadiites Basal spacinga(A) 17.0
Gallery heightb(A) 5.8
Surface area (m2/g) 587
Total pore volume c (cc/g) 0.60
Base catalyst
39.2
28.0
845
0.73
Acid catalyst
33.3
22.1
648
0.62
Catalyst No catalyst
a : Sample calcined at 538~ b : Gallery height = Basal spacing - 11.2 A (thickness of H-magadiite) [16]. c : Total pore volume obtained from Gurvisch rule [17] of nitrogen adsorption isotherm at 77K.
3.2.2 Silica-pillared kenyaite
The gelation of intercalated-TEOS by catalyst produces siloxane-intercalated derivatives with well-ordered basal spacings as well as the expansion of gallery height. The X-ray diffraction patterns and basal spacings of the products gelled by EtOH suspension, base-catalyzed reaction, and acid-catalyzed reaction are shown in Fig. 2(d, e, f), and Table 3, and these products exhibit reflections corresponding to basal spacings of 29.5, 39.9,, and 39.5 A, respectively. The silica-pillared products gelled by base- and acid-catalyzed reactions exhibits a large increase in the gallery height of 22.2 and 21.8 A, compared with the gallery height of the product gelled by EtOH suspension (11.8 A). A distinctive increase of the gallery height is related to the size and the structure of pillared silica, which could be associated with the amount of intercalated TEOS, the gelation condition (catalyst type, solvent composition, pH etc.), and the rate of gelation. Gelation by base and acid catalysts could minimize the release of TEOS outside the layered phase during the gelation of the intercalated TEOS, because gelation time is markedly reduced. The hydrolytic polycondensation of intercalated TEOS by acid or base catalyst could form silica clusters of highly branched and stiff network structure. These conditions could derive the effective gelation of intercalated TEOS in the interlayer, and contribute to develop the size and structure of pillared silica clusters which bring about the large expansion of the gallery height of pillared kenyaite. The adsorption/desorption isotherms of nitrogen were obtained at 77 K. Several pore characteristics calculated from them are listed in Table 3. The specific surface areas were calculated by BET equation from the adsorption isotherm below P/Po-0.1. The specific surface area of H-kenyaite shows the low specific surface area of 84 m2/g. The calcined silica-pillared products have high surface areas between 533-606 m2/g, depending on the catalyst types. The total pore volume of
59 Table 3 Physical properties of silica-pillared kenyaites Basal spacing a (A)
Galler~ height u (A)
Surface area (m2/g)
Total Micropore surface area c (m2/g)
Total pore volume (cc/g)
H-ke nyaite
18.0
0.3
84
56
0.10
No catayst
29.5
11.8
606
509
0.49
Acid catalyst
39.5
21.8
584
490
0.46
Base catalyst
39.9
22.2
533
427
0.52
Items
a : Sample calcined at 538~ b : Gallery height = Basal spacing - 17.7 A (thickness of H-kenyaite) [8]. c : Total micropore surface area obtained from t-plot of the nitrogen adsorption isotherm at 77K. base-catalyzed sample is the largest among three pillared samples, indicating that the average pore size of base-catalyzed sample is the largest. Fig. 3(b) shows the pore size distributions of silica-pillared kenyaites. The basecatalyzed sample shows a sudden increase in mesopore volume near 22A with a narrow pore size distribution relatively. The acid-catalyzed sample shows a narrow pore size distribution with a sharp peak near 18A. The abrupt gelation of acid and base catalysts is closely related to the formation of a more uniform pore. On the other hand, the sample gelled by the suspension of EtOH has a broader pore distribution and more microporosity (diameter < 20A). It is interesting that acid- and base-catalyzed products ae very similar in physical properties to surfactanttemplated mesoporous silica. 4. CONCLUSION The acid- or base-catalyzed reaction of hydrolysis and condensation polymerization of TEOS into a layered silicate gallery could affect the physical properties of silicapillared magadiite and kenyaite. The samples that were silica-pillared by acid- and base-catalyzed reactions shows a large increase in basal spacing. Also, they exhibit relatively narrow pore size distributions in the range of 18-40A and show high surface areas in the range of 533-845 m2/g, depending on types of the catalyst and layered silicate. These results indicate that the variations in the conditions of gelation contribute to improvement in physical properties of silica-pillared molecular sieves.
60
[ No Catalyst ~ -- - Base Catalyst - - - Acid Catalyst
o~ ~2
a
......... Acid - - - - EtOH Base
o'~' 1.0 "~u m0.8 ~ 0.6
N o 0.4 ~ 0.2 o i
20
i
i
i
I
40 60 80100
i
200
Pore Diameter, [.~,]
(a) Silica-pillared magadiite
0.0
i
i
10
i
i
i
i
i i I
I
I
i
1
100
Pore Diameter(~) (b) Silica-pillared kenyaite
Figure 3. Pore size distributions of silica-pillared products.
REFERENCES 1) K. H. Berke, W. Schwieger, and M. Porsch, Chem. Tech., 39 (1987) 459. 2) O.Y. Kwon, S. Y. Jeong, J. K. Suh, H. Jin, and J. M. Lee, J. Colloid and Interface Science, 177, JCIS PN 3928 (1995). 3) J. S. Daily, and T. J. Pinnavaia, Chem. Mater., 4 (1992) 855. 4) M. E. Landis, A. B. Aufdembrink, P. Chu, I. D. Johnson, G. W. Kirker, and M. K. Rubin, J. Am. Chem. Soc., 113 (1991) 3189. 5) R. Sprung, M. E. Davis, J. S. Kauffman, and C. Dybowski, Ind. Eng. Chem. Res., 29(1990) 213. 6) H. P. Eugster, Science, 157 (1967) 1177. 7) J. McAtee, R. House, and H. P. Eugster, Amer. Mineral., 53 (1968) 1026. 8) K. Beneke and G. Lagaly, Amer. Mineral., 68 (1983) 818. 9) R.A. Fletcher, and D. M. Bibby, Clays and Clay Minerals, 35 (1987) 318. 10) A. Brandt, W. Schweiger, and K. H. Bergk, Rev. Chem. Miner., 24 (1987) 564. 11) C. J. Brinker, and G. W. Scherer, "Sol-Gel Science The Physics and Chemistry of Sol-Gel Processing." Academic Press, London, (1990), P 97-160. 12) R. Aelion, A. Loebel, and F. Eirich, J. Am. Chem. Soc., 72 (1950) 5705. 13) M. Nogami, and Y. Moriya, J. Non-Crysralline Solids, 37 (1980) 191. 14) J. H. Boer, B. G. Linsen, T. V. D. Plas, and G. J. Zondervan, J. Catalysis, 4 (1965) 649. 15) P. B. Barrett, L. G. Joyner, and P. P. Halenda, J. Am. Chem. Soc., 73 (1951) 373. 16) G. Lagaly, and K. Beneke, American Mineralogist, 50 (1975) 650. 17) L. Gurvitsch, J. Phys. Chem. Soc. Russ., 47 (1915) 805.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
61
A New Synthetic Route and Catalytic Characteristics of Pillared Rectorite Molecular Sieves
Jingjie Guan Zhiqing Yu Zhenyu Chen Liwen Tang and XieqingWang Research Institute of Petroleum Processing, China Petro-Chemical Corporation
This paper presents a new synthetic route and catalytic characteristics of pillared rectorite molecular sieves (PR-MS).
The PR-MS was prepared with aluminum pillaring
agent improved by poly (vinyl alcohol) according to route of mixing, drying to take shape, washing, and calcination.
It has wide pore structure with basal spacings of 27-30 ,~.
Under same conversion their activity for cracking heavy oil is 3-4 wt % higher and total yields of gasoline and light cycle oil are 6-7 wt % higher than that of commercial cracking catalysts containing USY zeolites. The catalysts developed from the PR-MS and Y-zeolites have high catalytic activity and low bottom yield. The PR-MS has also good light olefin selectivity. The catalysts containing the PR-MS and ZSM-5 type molecular sieves are a class of cracking catalysts for maximizing olefin production.
1. INTRODUCTION It is an important way for developing new energy resources to convert more heavy oil into liquid petroleum gas, gasoline and light cycle oil products. Although Y-type zeolites are commercially widely used as cracking catalysts their pore sizes are within the limits of less then 9,~. The pore sizes are not effective for cracking reactants with large molecule sizes. There is a need for new molecular sieves that are able to crack heavy oil and are easy to be commercialized in catalyst manufactory industry. Al-pillared rectorites developed by RIPP in 1985 are a class of new pillared clay molecular sieves [1]. The molecular sieves have excellent hydrothermal stability, solid acid sites and greater versatility than that of the faujusite [2]. These characteristics are advantageous for cracking heavy oil feedstock. However the prior pillared clay molecular sieves were prepared according to route of pillaring reaction of thin clay slurry and A1pillaring agent, washing, filtering, drying and calcination [3]. In general the clay particles are less than 2 mi'cra that are difficult to be filtered in commercial scale. In 1991 to tackle
62 the filtering problem a synthetic method without filtering operation of thin clay slurry was provided. However catalytic activity of the catalysts prepared by the method is not as good as Y-zeolite catalysts. For example, under same evaluated conditions by riser pilot unit the conversions of the two catalysts are 63 wt % and 67 wt % respectively [4] Up to now the pillared rictorite catalysts have not been used in FCC process. The object of this paper is to present a new synthetic route and catalytic characteristics of PR-MS with high catalytic activity. On the basis of direct research possibility of developing the PR-MS into commercial molecule sieves and microspheric cracking catalysts is studied. 2. EXPERIMENTAL 2.1 Synthetic routes of samples
Raw clays used for preparing samples are naturally rectorites with regularly interstratified mineral structure. Their quality specifications are conformable to properties in Table 1-2. Table 1 Physicochemical properties ofthe rectorites D001 by X-ray method /~
Cation exchange capacity meq/100g ....
Phase transformation temperature oC
23-24
40-60
1050
Table 2 Chemical composition of the rectorites Item Contents
_
Na20
CaO
Fe203
A!203
SiO2
wt %
1.2-2.0
3.5-6.0
< 1.5
39-43
43-51
Pillaring-bonding agent used for preparation of samples is Al-sol solution improved by poly (vinyl alcohol) (abbreviated PVA). Its 27NMR spectra are shown in Fig. 1. The PR-MS and catalysts containing PR-MS and other zeolite components were prepared by synthetic route A in Fig. 2 according to operation conditions reported in the literature [5]. The prior pillared interlayer rectorites (PIR) were prepared by conventional method [6] in accordance with synthetic route B in Fig. 2.
63
~.~ lOO
. . .~! ,~, ,~,~.~,
........ 50
0
-50
ppm
Figure 1 27NMR spectra of AI- pillaring-bonding agent
=---H ....
Rectorites Pillared-bonding agent Other composition ,.
H
Mixingand drying to take shape
Wa,shingFiltering of microspheric
m
Drying ..Samples Calcination
A: Synthetic route of the PR-MS and related catalysts
Rectorites-~
H Filteringof H Washing, .... FilteringU.... Drying
Pillaring
Pillaring agent..I I reaction
clay slurry
of clay slurry
..Samples
] i Calcination
B: Synthetic Route of the prior pillared rectorites Figure 2 Principle scheme of sample preparation It can be seen that in the prior PIR sample preparation special pillaring reaction is involved and the filtertion of clay slurry is difficult. However in the PR-MS preparation the special pillaring reaction operation required in prior art has been omitted because pillaring reaction can be completed in presence of PVA during mixing process prior spray drying. Also the pillaring agent improved by PVA is not only good pillaring agent used in thick clay slurry but also good bonding agent. The reaction mixture of the pillaring agent and clay is directly dried to take shape without filtering operation for fine clay slurry. It is easy to be produced in commercial scale. Besides this, it can contain other bonding agents required for preparing microspheric samples. Therefore, the new synthetic route can be used for preparation of microspheric cracking catalysts containing the PR-MS and other molecular sieves as well as the PR-MS
2.2. Physicochemical analysis 27NMR spectra were obtained by using Bruker Am-300 with operation conditions of SW-25000HZ SI=4K DE-300 LB=30 AQ-0085 RD--0.25 PW=3.
64 X-ray diffraction measurement was obtained by using Geigerflex D-9C X-ray diffractometor at a scan rate of 2~ 0/min and with monchromatic Cuka radiation. Surface areas and pore volumes were measured by using BET method from nitrogen adsorption isotherms. 2.3. Catalyst testing
Microactivity test was used for evaluating catabr characteristics of samples. The samples were deactivated at 800~ for 4 hours with 100% steam before evaluation. Catalytic activity for cracking light gas oil (235-337~ operation conditions of reaction temperature of 500 ~ (WHSV) of 16hr-1 and catalyst to oil ratio (c/o) of 3.2. Catalytic activity for cracking heavy oil (330-520~ conditions of reaction temperature of 520~
was obtained according to weight hourly space velocity
was evaluated by
operation
WHSV of 16hr-: and C/O of 3.0.
3. RESULTS AND DISCUSSION 3.1. Evaluation of new synthetic route
The chemical composition, physico-chemical properties and X-ray diffraction pattern of the PR-MS samples are shox~ Table 3-4 and Fig. 3. Table 3 Chemical composition of the PR-MS Contents Samples . . . .
wt %
Na20
CaO
Fe203
A1203
SiO2
The PR-MS
1.5
3.9
0.9
49.8
44.6
The prior P,IR
1.5
3.3
1.3
48.5
42.5
Table 4 Surface areas and pore volumes of the PR-MS Samples
Surface areas m2/g Fresh Steamed at
pore volumes ml/g Fresh Steamed at
800~ for 4hrs
800~ for 4hrs
The PR-MS
145
127
0.12
0.10
The prior PIR
144
101
0.13
0.10
65
29A
29A
=o cD
27/~
.>.
..>
3
I~
l
I
2 Theta
2 Theta
A: Sample prepared by present work
B: Sample prepared by prior method
Figure 3. X-Ray diffraction patterns of pillared rectorites 1" fresh sample. 2" sample steamed at 800~ for 4 hrs The results from Table 3-4 and Fig.3 indicate that the PR-MS prepared by new synthetic route in present work has physicochemical properties similar to prior PIR. The PR-MS has basal spacing of 29/~ for fresh samples and basal spacing of 27,~, for samples steamed at 800~ for 4 hrs that is the same as prior PIR, Especially, the height of d 001 peak for the PR-MS is higher than that of prior PIR indicating that a class of good pillared clays can be obtained by the simplified preparation method in present work. The new synthetic route of pillared clays and related catalysts has a bright future for commercial production. Catalytic activity of the PR-MS as compared with prior PIR is listed in Table 5. Table 5 Catalytic activity of samples for cracking light gas oil The PR-MS at present work
The prior PIR
Samples
Commercial USY catalyst
Microactivi~ %
75
71
72
66 The data in Table 5 indicate that PR-MS has microactivity of 75 wt % versus microactivity of 71 wt % by prior PIR and microactivity of 72 wt % by commercial USY catalysts.
It
means that catalytic activity of the PR-MS prepared by the new synthetic route is higher than that of prior PIR and commercial USY catalysts. It fully proves that the new synthetic route provided in present work is successful for preparing
pillared clays and related
catalysts.
3.2. Catalytic properties of the PR'MS and catalysts containing the PR-MS 3.2.1 Reaction characteristic for cracking heavy oil The activity and selectivity for crackling heavy oil with the PR-MS and catalysts containing the PR-MS and Y zeolites as compared with commercial USY catalysts are shown in Table 6. Table 6 Activit), and selectivity of th e PR-MS for cracking heavy oil Conversion Samples
Yield ,,.
wt
%
LCO
Bottom
wt %
Gas
Coke
Gasoline
USY catalysts The PR-MS
77.2
21.3
2.1
53.8
12.9
9.9
.at present work
77.4
16.1
4.7
56.6
16.4
6.2
The catalyst containing PR-MS and Y zeolites
81.8
22.3
3.6
55.9
13.8
4.4
Commercial
The data from Table 6 indicate that in cracking reaction with commercial USY catalysts a 9.9 wt% of bottom are remained but in the same operation conditions with the PR-MS and their catalysts only 6.2 wt % and 4.4 wt % of bottom are remained respectively. Obviously the PR-MS and its catalysts have catalytic activity for cracking heavy oil much better than that of the commercial USY catalysts. Also under almost same conversion level (77.2-77.4 wt %) the PR-MS yields gasoline of 56.6 wt % and light cycle oil of 16.4 wt % versus gasoline of 53.8 wt % and light cycle oil of 12.9 wt % by commercial USY catalysts indicating that the PR-MS has good gasoline and light cycle oil selectivity. The results are corresponding to wide pore structure of the PR-MS which is favored for cracking reactants with large size molecules.
67 3.2.2 Reaction characteristic for maximizing olefin production. The olefin selectivity of the PR-MS catalysts as compared with commercial REHY catalysts are listed in Table 7. Table 7 Light olefin selectivity of the PR-MS and for cracking heavy oil Samples Evaluation conditions
Conversion
wt %
Catalyst-1 REHY+Matrix
REHY+PR-MS
520~ C/O 3 WHSV 16-1
520~ C/O 3 WHSV 16-1
71
.Catalyst-3 ZSM-5+PR-MS 520~ C/O 4.5 WHSV 16-1 J
73
71
20.2 2.8 47.9 15.3 13.8
17.5 4.1 51.2 16.8 10.4
38.1 2.4 30.5 16.9 12.1
C~
0.8
0.6
1.7
C4
4.1
4.4
14.5
C5 C2 "C5
5.4
6.5
15.0
3.4 13.7
5.5 17.0
8.5 39.8
1.2
1.7
6.1
2.0
3.1
5.8
3.2
4.8
11.9
Product yield wt % Gas Coke Gasoline Light cycle oil Slurry Olefin yield wt%
iC] iC~
yield wt %
iC~-iC5
The data from Table 7 indicate that the PR-MS has not only high capability for converting heavy oil but also good light olefin selectivity. Under almost same conversion level (71-73 wt %) the catalyst-2 containing the PR-MS and the REHY zeolites has C:-C5 yield of 17 m
wt % and iC4-iC5 yield of 4.8 wt % but catalyst-1 containing only the REHY zeolites as active composition has C, -C5 yield of 13.7 wt % and iC4-iC~ yield of 3.1 wt %. It means that the light olefin selectivity of the PR-MS components is better than that of the Y-type
68 zeolites. Catalyst-3 developed from the PR-MS and the ZSM-5 type zeolites have the best light olefin selectivity in the three samples. It has C2 "C5 yield of 39.8 wt % and iC~-iC~ yield of 11.9 wt %. Obviously, the catalysts containing the PR-MS and ZSM-5 zeolites are a class of cracking catalysts for maximizing olefin production. The results above mentioned have clearly demonstrated that the PR-MS is both active components like molecular sieves and high activity matrix composition of catalysts. It can be used for preparation of cracking catalysts to convert more heavy oil .into light olefins gasoline and light cycle oil products.
4. CONCLUSION 1 The pillared rectorite molecular sieves (PR-MS) and related catalysts with high catalytic activity can be obtained by special Al-pillaring agent according to synthetic route of mixing, drying to take shape, washing and calcination. The preparation procedures are easy to be put into effect in commercial scale. 2 The PR-MS and microspheric cracking catalysts developed from the PR-MS and Yzeolites have high catalytic activity for cracking heavy oil and good selectivity of gasoline and light cycle oil. It is much better than that of commercial USY microspheric catalysts. 3 The PR-MS has better selectivity of light olefins than that of Y-zeolites. The catalysts containing the PR-MS and ZSM-5 type zeolites are a class of new cracking catalyst for maximizing light olefin production. REFERENCES !. 2. 3. 4. 5. 6.
Jingjie Guan; Enze Min and et al, Proceeding 9th International Congress on Catalysis Vol. 1, p104-111. Calgary, Canada ,(1991 ). Jingjie Guan and Thomas J. Pinnavaia, Abstract Proceeding International Symposium on Soft Chemistry Routes to New Materials in Nantes,France (1993). N. Lahav, U. Shani and J. Shabtai, Clays and Clay Minerals, Vol. 26, No. 2, p107-115 (1978). Jingiie Guan and et al , Proceeding of the International conference on Petroleum Refining and Petrochemical Processing, Beijing, P.R.China Vol. 3, p1255 (1991). C.N. 92114024 X (1995) U.S.Patent 4,757,040 (1988)
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
69
Textural Control of M C M - 4 1 Aluminosilicates Francesco Di Renzo, Nicole Coustel, Miren Mendiboure, H616ne Cambon and Franqois Fajula Laboratoire de Mat6riaux Catalytique et Catalyse en Chimie Organique, URA 418 du CNRS, Ecole Nationale Sup6rieure de Chimie de Montpellier, 8 rue de l'Ecole Normale, 34053 Montpellier, France, fax (33)67144349
The thickness of the walls between mesopores in MCM-41 sieves can be controlled by modifying the solubility of silica and aluminosilicate species, notably by changing the alkalinity of the synthesis system. This effect strongly influences the thermal stability of aluminosilicate MCM-41 in activation conditions.
1. INTRODUCTION The disclosure of the properties of micelle-templated mesoporous silicas [1-3] has represented a twofold breakthrough. From the point of view of the materials scientist, it has marked the starting point of a blossoming research on the selforganization of inorganics and surfactant molecules [4-6]. From the point of view of the catalysis and sorption technologist, it has fullfilled a long expectation for solids with custom-tailored uniform pores of size larger than the micropores of zeolites [7]. The pore size is easily controlled by choosing a surfactant able to form micelles of the required diameter. For instance, the diameter of the hexagonally-packed cylindrical pores of MCM-41 silica can be adjusted at any value in the 18-37 A range by incorporating alkyltrimethylammonium ions with hydrocarbon chains ranging from 8 to 16 carbons [2]. Less attention has been paid to another textural parameter of the MCM-41 honeycomb: the thickness of the silicate walls which separate the micelles of the as-synthesized material and the mesopores of the activated sieve [8]. Molecular
70 dynamics simulations have shown this parameter to control the stability of the MCM-41 framework [9]. This communication deals with the correlations between the synthesis and activation parameters and the texture of the final mesoporous sieve, and the informations thereby provided about the mechanism of self-assembly of cationic surfactant and silicates.
2. E X P E R I M E N T A L
MCM-41 aluminosilicate samples were prepared from synthesis systems of composition xNa20 2.8CTMA20 A1203 55SIO2 1800H20, where CTMA stands for cetyltrimethylammonium. The samples were numbered from 1 to 6 in the order of increasing
alkalinity,
expressed
as
[(Na++CTMA+-AI(OH)4-Br-2SO42")/SiO2].
Alkalinity values of the synthesis mixtures are reported in Table 1. Reagents were mixed with stirring at 70~
in the order:
deionized water,
NaOH
(SDS),
AI2(SO4)318H20 (Rh6ne-Poulenc Prolabo), CTMABr (Aldrich), precipitated silica (Rh6ne-Poulenc Zeosil 175MP, 175
m2/g, grain
wt%). The gel was heated up to 120~ autoclave, kept 15 minutes at 120~
size 2-201.t, Na 0.07 wt%, AI 0.17
in 1 hour in a 130 ml stirred stainless steel
and rapidly cooled down.
Table 1 Alkalinity of the synthesis medium and properties of mesoporous aluminosilicates.
Sample OH-/SiO2
a~ A
a550 A
AW<373K AW>373K p/po
Vmp
SBET
Woo
ml/g
mE/g
Woo
AI (Si+AI)
1
0.02
no MCM-41 formed
2
0.14
57
52
0.08
0.39
0.38
0.49
630
0.031
3
0.29
54
48
0.12
0.56
0.36
0.66
860
0.042
4
0.40
51
47
0.05
0.59
0.33
0.73
960
0.050
5
0.52
50
44
0.10
0.74
0.32
0.82
1090
0.069
6
0.65
49
44
0.12
0.77
0.28
0.55
940
0.083
71 The products,
washed with water and ethanol and dried at 80~
were
characterized by powder X-ray diffraction (XRD, CGR Th6ta 60 diffractometer, 0.25 mm slits, monochromated Cu Kt~ radiation), scanning electron microscopy (SEM) and electron probe microanalysis (EDX) (Cambridge Stereoscan 260 apparatus), thermal gravimetry (TG, Setaram B85 instrument, air flow, 15 mg samples, heating rate 5 K/rain), and N2 sorption at 77K (Micromeritics ASAP 2000C, 250~ 850~
outgassed samples) after calcination at temperatures in the 550-
range (air flow, heating rate 1 K/rain, 8 hours isotherm).
3. RESIILTS In Figure 1 a typical XRD diagram is reported, showing a peak slightly above 1 ~
with a width at half height of 0.4 ~
and a broad band centered around 2 ~
The two features correspond, respectively, to the 100 line and to the convolution of the 110 and 200 lines of a MCM-41 structure with low long-range order [10, 11]. The parameter a of the hexagonal lattice of all samples as synthesized and after calcination at 550~
are reported in Table 1. A shrinking of the hexagonal
cell with calcination is observed, as a decrease of the lattice parameter for the samples prepared at higher alkalinity. Intensities of the XRD lines significantly increase with calcination, probably due to the better contrast which results from
Figure 1. X-ray diffraction diagram of sample 3 after calcination at 550~
,,~1,,,i,,,i,~,1,~,1,,,i,,,i,,,i,,,i,,~1,,,
1
2
Theta Degrees
72
the extraction of the organic phase. The TG patterns are in good agreement with literature reports [3] which allow to attribute the weight loss below 100~ above 100~
to water desorption and the weight loss
essentially to the degradation and extraction of the organic phase.
Weight losses below and above 100~
expressed as fractions of the final mass are
reported in Table 1 for all MCM-41 samples. The weight loss corresponding to the surfactant decomposition is larger for samples prepared at higher alkalinity. In Figure 2 the isotherms of N2 sorption at 77 K are reported for a typical sample after calcination at 550 and 850~
(Figures 2a and 2b, respectively).
Sorption curves are typical type IV isotherms [12] without any hysteresis below p/po 0.9. The sorption step in the p/po range 0.3-0.4 is sharp for the samples calcined at 550~
(Figure 2a), indicating a narrow pore size distribution. The step
of the isotherm is less sharp and shifted to a lower pressure for the samples
700
Figure 2. Nitrogen sorption
600 n CO
400
o
300
O W
m
nt (D c0 Q
.2 0
/
500
c~
%, 0
-f
200 100
f
isotherms at 77K for sample
J
3 calcined at 550~
a) and 850~ (curve b). (+) adsorption, (*) desorption.
0
600 500 400 300
-//
f
200 100
0
~
0.0
~
I
T
0.2 RELATIVE
(curve
t
0.4
1
T ~ T
r
0.6
PRESSURE
0.8 ,
(P/Po)
I
73 calcined at higher temperature (Figure 2b), indicating a broader size distribution of mesopores with a smaller average diameter. The isotherm of sample 6 already features a less sharp sorption step after calcination at 550~ The partial pressure of the sorption step is reported in Table 1 for all samples calcined at 550~
as the mesopore volume evaluated at the top of the step and the
surface area from the BET equation for P/P~
The partial pressure of the
sorption step slowly decreases as the alkalinity of the synthesis system increases. Mesopore volume and surface area increase at increasing alkalinity up to a maximum at a OH/SiO2 0.5, and decrease for further increases of alkalinity. The c parameters of the BET equation are 102+5 for samples calcined at 550~ and 62+10 for samples calcined at 850~
A significant sorption takes place
beyond the filling of mesopores, in the partial pressure range 0.4-0.9, suggesting a large outer-surface area for the MCM-41 grains. The t-plot of the data of Figure 2a is reported in Figure 3. It indicates that no micropores are present (absence of downward deviation) [13] and confirms that capillary condensation takes place in mesopores with narrow size distribution. The gentle slope of the t-plot beyond the capillary condensation step corresponds to sorption on the outer surface of the mesoporous grains. SEM of all samples shows large aggregates of less than 100 nm grains. The aluminium mole fraction measured by EDX is reported in Table 1 for all samples. The aluminium content increases at increasing alkalinity of the synthesis medium.
EL i-O3
000 00
400 121 \ o o
0 W
m [~ o LO n CE
-
Figure 3. t-plot for the N2 sorption isotherm at 77K of sample 3 calcined at 550~
200
1 lZllZl
_J 0
IZl
-
!
IZI
1
u... t-HARKINS
i
i
i
1
4 ,~, J U R A
b ~.
(A
74 4. DISCUSSION The alkalinity of the
synthesis
system affects
several properties
of the
surfactant-silicate assembly. For any alkalinity value high enough to satisfactorily dissolve the source of silica, materials corresponding to the definition of MCM-41 sieves [14] are formed. The width of the XRD peaks does not correspond to a wide pore size distribution, suggesting that the lumping of the 110 and 200 peaks in one broad signal corresponds to a lack of long-range order, in agreement with the observed size of the MCM-41 grains, no larger than a score of lattice patterns. The small grain size can be accounted for by heterogeneous nucleation of MCM41 on colloidal silica [ 15]. In Figure 4 the values of the lattice parameter a and the CTMA content of the as-synthesized MCM-41 samples are reported as a function of the alkalinity of the synthesis medium. As alkalinity increases, the lattice parameter a, corresponding to the distance between micelle axes, decreases from 57 to 49 /~, while the CTMA/SiO2 mass ratio increases from 0.39 to 0.77. A simultaneous increase in the organic fraction and decrease of the distance between micelle axes corresponds to a lower volume fraction occupied by silica, hence to thinner walls between micelles. A simple geometric model, assuming hexagonal pore section [16], CTMA density equal to the density of hexadecane (0.77) and amorphous silica density 2.2 [17], allows to calculate the average wall thickness t. The calculated t values, reported in Figure 4, regularly decrease at increasing alkalinity and account for the observed decrease of the lattice parameter a. The micelle diameter of the as-
e.....
Fig. 4. Lattice parameter a ( 9 ), 1.0
50
.<
U
f
0.5
10. . . . OH'/tSi02
015
'
wall thickness t ( A ) , O b5 < I-"
o
and organic
mass fraction ( O ) of MCM-41 as a function of the alkalinity of the synthesis medium.
75 synthesized samples can be considered as independent of the alkalinity. The solubility of silica rapidly increases with alkalinity [18], whereas most aluminate reacts with excess silica in the whole synthesis field to form less-soluble aluminosilicate. As a consequence, the higher the alkalinity the higher the amount of soluble silica left in the solution at the end of the synthesis, and the higher the aluminiun content of the solid product. This result implies that the silicate coating of each micelle tends to be at the equilibrium with the surrounding solution throughout the precipitation of MCM-41, and strongly supports a mechanism of formation by self-assembly of inorganic-coated micelles [4]. The solubility of silica is the main factor which influences the equilibrium between silicate coating and solution, and the wall thickness depends on the ratio between the amount of outof-equilibrium
silicate
and the
area
of the
micellar
surface
available
for
condensation. The wall thickness significantly influences the thermal stability, as indicated in Figure 5, where the results of N2 sorption on MCM-41 calcined at 550~
are
reported as a function of the organic fraction in the parent material. The mesopore volume is proportional to the organic volume fraction and the pore diameter is nearly constant for all samples with walls thicker than 8 A. For all these samples, it can be assumed that calcination at 550~
has not altered the basic geometry of
MCM-41. In the case of sample 6, with average wall thickness lower than 8 A_, the pore volume and diameter are much lower than expected, and the pore size
.___e_._.=__.
Fig. 5. Mesoporous volume (O) and average pore diameter ( & ) 30
MCM-41
calcined at 550~
as a
function
of
mass
the
organic
fraction of the as-synthesized solid.
0.5
20 "4
10
E 01/ 0
of
!
CTMA/SiO 2
0.5
76 distribution is wider than for the other samples, indicating that the material has already begun to sinter in the activation conditions at 550~ REFERENCES
1. 2.
T. Yanagisawa, T. Shimizu, K. Kuroda & C. Kato, Bull. Chem. Soc. Jpn 63 (1990) 988. C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli & J.S. Beck, Nature 359 (1992) 710.
3.
J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T.W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins & J.L. Sehlenker, J. Am. Chem. Soc. 114 (1992) 10834.
4.
C.Y. Chen, S. Burkett, H.K. Li & M.E. Davis, Microporous Materials 2 (1993) 27.
5.
Q. Huo, D.I. Margolese, U. Ciesla, P. Feng, T.E. Gier, P. Sieger, R. Leon, P.M. Petroff, F. Seh~th & G.D. Stucky, Nature 368 (1994) 317.
6.
7. 8.
A. Firouzi, D. Kumar, L.M. Bull, T. Besier, P. Sieger, Q. Huo, S.A. Walker, J.A. Zasadzinski, C. Glinka, J. Nicol, D. Margolese, G.D. Stucky & B.F. Chmelka, Science 267 (1995) 1138. D . E . W . Vaughan, Studies in Surface Science and Catalysis 49 (1989) 95. N. Coustel, F. Di Renzo & F. Fajula, J. Chem. Soc. Chem. Commun. 1994, 967.
9. 10.
B.P. Feuston & J.B. Higgins, J. Phys. Chem. 98 (1994) 4459. P.T. Tanev & T.J. Pinnavaia, Science 267 (1995) 865.
11. 12.
C.Y. Chen, S.Q. Xiao & M.E. Davis, MicroporousMaterials 4 (1995) 1. S. Brunauer, L.S. Deming,W.S. Deming & E. Teller, ,LAmer. Chem. Soc. 62 (1940) 1723.
13.
J.H. de Boer, B.G. Linsen & Th.J. Osinga, J. Catal. 4 (1965) 643.
14.
J.S. Beck, C.T.W. Chu, I.D. Johnson, C.T. Kresge, M.E. Leonowicz, W.J. Roth & J.C. Vartuli, WO pat. 91/11390 (1991).
15.
J. Liu, A.Y. Kim, J.W. Virden & B.C. Bunker, Langmuir 11 (1995) 689.
16.
V. Alfredsson, M. Keung, A. Monnier, G.D. Stucky, K.K. Unger & F. Schtith, J. Chem. Soc. Chem. Commun. 1994, 921.
17. R.K. Iler, The chemistry of silica, Wiley, New York 1979, 22. 18. Ref. 17, 126.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
77
N e w routes for synthesizing mesoporous material Yan Sun a, Wenyong Lin a, Jiesheng Chen a, Yong Yue b, and Wenqin Panga* aKey Laboratory of Inorganic Hydrothermal Synthesis, Department of Chemistry, Jilin University, Changchun, 130023, P.R. China bWuhan Institute of Physics, Academia Sinica, Wuhan, 430071, P.R. China New routes including direct thermal treatment, room-temperature crystallization and microwave heating were developed for the formation of mesoporous material MCM-41, and the properties of the materials from these new routes were compared with MCM-41 hydrothermally synthesized. The pore sizes of the MCM-41 materials are normally distributed with an effective pore diameter that falls into the range of 20-40 A. An unusual product which possesses a bimodal mesopores distribution was obtained from wet-gel thermal treatment with no presence of any auxiliary organic molecules. The well-defined smaller pores are around 30 A in diameter, and the large pores are within the range 80-200A MAS NMR spectroscopy reveals that after calcination to remove the organic template in the AIcontaining MCM-41, a small part of the tetrahedrally-coordinated framework aluminum atoms become octahedrally-coordinated and a considerable amount of Si-OH species are generated.
1. INTRODUCTION In 1992 novel mesoporous molecular sieves designated as MCM-41 were reported by Mobil scientists[I-4].. These materials possess hexagonally arranged unidimensional pores, the size of which can be tuned within 20-100 A by varying the preparation conditions. Unlike other mesoporous materials such as intercalated clays, the pore size of an MCM-41 molecular sieve is considerably uniform, and its uniformity is comparable with that of microporous crystalline materials. The MCM-41 materials were normally obtained by hydrothermal preparation and their structures were found to be constructed mainly from amorphous inorganic silica walls around surfactant molecules. By adding guest molecules such as mesitylene into the synthesis system, MCM-41 samples with larger pore sizes can be obtained. However, the pore size of MCM-41 materials is affected by other factors as well.
78 Several mechanisms for the hydrothemml formation of MCM-41 have been proposed in the literature [5-8]. To further the understanding of the formation of MCM-41 molecular sieves, we investigated the factors that afti~ct the hydrothermal synthesis of these materials, and new synthetic routes other than the hydrothermal one have been developed. It is the purpose of this paper to describe the new routes to the formation of MCM-41 materials and its properties in comparison with the MCM-41 synthesized hydrothermally. 2. EXPERIMENTAL
2.1 Materials and Samples preparation 1. Hydrothermal synthesis of MCM- 41.
Sodium hydroxide, distilled water and a
surfactant C,H2,+I(CHa)3Nx(X=CI, Br; n=12, 16) were mixed with or without mesitylene (MES). Then the sodium aluminate solution was dropped in to the mixture with stirring. When the mixture became homogeneous, Aerosil (99% SiO2) or tetraethyl orthosilicate (TEOS) was added. The final reaction gel Was loaded in a PTFE-lined stainless steel autoclave followed by heating at 110-160 ~
for 1-7 days. The product was recovered by
filtration, washed with water and dried at ambient temperature. The as-synthesized samples were calcined at 550~ for 5 hours to obtain the template-free MCM- 41 materials. 2. Room-temperature crystallization of MCM-41. This synthetic route involved tetraethyl orthosilicate exclusively as the silicon source. H20, a surfactant and TEOS were mixed and stirred until homogeneous. To this mixture, either NaOH or hydrochloric acid was added followed by stirring for 30 minutes. The solid product was filtered, washed with water and dried at ambient temperature. 3. Thermal formation of MCM-41. There are two sub-routes for the thermal formation of MCM-41. The wet-gel route is as follows: NaOH, H20, a surfactant and tetraethyl orthosilicate were mixed with stirring for 2 hours. The mixture was transferred int6 a crucible followed by heating at 550~ in an oven for about 1 hour. Another sub-route is the precursor route: an amorphous solid precursor obtained by drying a hydrothermally treated gel was heated at various temperatures in an oven and the products were subjected to XRD Characterization. The gel used for the hydrothermal treatment was prepared in a way similar to that for the hydrothermal synthesis of MCM-41. 4. Microwave synthesis of MCM-41. Homogeneous reaction mixture containing NaOH, H20, a surfactant, the silicon source with or without NaAIO2 was sealed in a cylindrical PTFE container followed by heating in a 650W microwave oven for 1-30 rain. The solid product was recovered by filtration and dried at ambient temperature.
79
2.2 Characterization techniques X-ray powder diffraction patterns were obtained on a Scintag XDS-2000 diffractometer with Cu KGt radiation. The 20 scanning speed was 0.5~ The scanning electron micrographs were taken on a Hitachi X-650B scanning electron microscope. An ASAP 2400 automatic adsorption instrument was used to perform the N2-adsorption and the pore size distribution measurements, and a Bruker MSL-400 NMR spectrometer was used to record the 27A1 and 29Si NMR spectra. Cross-polarization technique was applied to obtain the 29Si NMR signals. 3. RESULTS AND DISCUSSION With Aerosil as the silicon source, the XRD patterns of products depend on the H20/SiO/ ratio in the reaction mixture. If H20/SIO2>80, a lamellar phase or a MCM-41 sample (designated MCM-4 l-A) with a well-defined XRD pattern showing the (100), (110), (200), and (210) reflection is. readily formed. However, when the H20/SiO2 falls into the range between 10-70, a mesoporous material (denoted MCM-41-B) which exhibits a strong broad XRD reflection at a 20 angle lower than 2 ~ and a weak one at around 3.5 ~ was obtained (Fig. l b). The typical gel composition for synthesis is shown in Table 1. By varying the synthetic
500~ C 400"C 250~ MCM-41-A 175~ without treatment MCM-41-B
2.0
4.0
6.0 20, o
Fig. 1 XRD patterns of MCM-41-AI and B2.
8.0
2.0
4.0
6.0
8.0
10.0
20, ~ Fig. 2 XRD patterns of typical solid precursor treated at different temperature for l h.
80 Table 1. Gel compositions and synthetic conditions for MCM-41 materials Sample
Gel composition a
Reaction
pH
temp(~
Reaction time (Hs)
MCM-4 I-A 1
0.06AlzO3:SiO2:0. 5( 16Br):0.18Na20:107H20
140
11
72
MCM-4 i -A2
0.05A1203:SIO2:0.25(16CI):0.23Na20:107H20
140
!1
72
MCM-4 ! -B 1 MCM-4 ! -B2
0.04AlzO3:SiO2:0.25(l 2CI):0.30Na20:30H~O
150
12
72
0.04A1203:SIO2:0.47(16CI):0.65Na20:23H~O
150
11
72
MCM-41-Cl MCM-4 ! -C2
SIO2:0.09(16C!):0.13(TMA)20: ! 8H20 SIO2:0.09(16CI):0.13(TMA)20:0.4MES: 18H20
150 ! 50
13 13
1 I
MCM-41-D1
TEOS:0.1 (16Br):(0.23-0.47)NazO: 118H20
-25
>10
0.5-10
MCM-41-D2
TEOS:0. i 3(16Br): 12HCI:94H20
-25
<1
0.5-5
MCM-41 -E MCM-41 -F 1
TEOS:0.63(I 6CI):0.23Na20:65H:O
....
11
TEOS:0.2(I 6C!):0.03Na20:71HzO TEOS:0.4(I 6Ci):0.05Na20:9 i HzO
550 550
11 11
MCM-41 -F2
0.2 72 72
"~16Br=C16H33(CH3)3NBr, 16CI=CI6H33(CH3)3NCl, 12Ci=CI2H25(CH3)3NCI conditions, the main peak for MCM-41-B shifts between 1.3 ~ and 2.0 ~ The chain length of the surfactant used for the preparation has no distinct effect on the d-spacing of the (100) reflection. A similar phenomenon was observed previously by Tanev et al.[9]. On the other hand, the addition of mesitylene into the reaction mixture invariably increases the d-spacing of the main peak. After calcination, the main peak for all MCM-41 materials shifts toward higher 20 angle and the maximum shift observed reaches 7 A ind-spacing. It is very interesting that some amorphous solid precursors, which were produced by hydrothermal treatment of gels with HzO/SiOz<80 at 100-140~ can be transformed into crystalline MCM-41 (designated MCM-41-C) after direct calcination at elevated temperatures. If the H20/SiOz ratio is larger than 80 in the initial reaction gel, the recovered amorphous precursors remain non-crystalline after the thermal treatment. Fig. 2 shows the effect of the thermal treatment temperature on the transformation of typical amorphous solid to MCM-41-C. It is seen that at 175~ the XRD-amorphous phase starts to gain some c.rystallinity and at 250~ the crystallinity increases greatly. At 500~ the product reaches its maximum. The formation of the crystalline MCM-4 I-C from an amorphous precursor is probably due to the rearrangement of the disorderly-placed inorganic walls in the precursor. With an appropriate gel composition, MCM-41 can be prepared at room temperature. The reaction mixture for room temperature preparation is either alkali (pH>10) or acidic (pH<_l), and TEOS is preferably used as the silicon source. To obtain highly crystalline MCM-41, the reaction mixture must be kept under stirring for at least 30 minutes, and longer crystallization times have no further effect on the Crystailinity of the product. The incubation probably helps the hydrolysis and the polymerization of the SiO44- species in the reaction mixture. The XRD pattern of the MCM-41 material (designated MCM-41-D) prepared at room temperature is similar to that for MCM-4 l-A, suggesting that as long as the ratio of H20/SiO2 falls into a
81 certain range, the variation of crystallization temperature has no influence on the formation behavior of MCM-4 I. Nowadays, microwave heating technique has been widely used for inorganic and organic synthesis. The microwave synthesis of zeolite-A, X, analcime and other crystalline microporous materials also appeared in the literature[10]. We investigated the microwave synthesis of mesoporous materials and found that it is an effective route to obtain highly crystalline MCM-41 (denoted as MCM-41- E). The typical preparation of MCM-41 takes only 15 minutes of microwave heating time using a 650W microwave oven whereas a similar reaction gel takes 1 day to form crystalline MCM-41 under hydrothermal preparative conditions. All the reaction gels used for microwave treatment are amorphous on the basis of XRD patterns, excluding the possibility that crystalline MCM-41 is formed before the microwave treatment. For the wet-gel thermal formation of MCM-41, the amorphous gel should be prepared from TEOS, and the room-temperature aging time (with stirring) also plays a key role in the formation of crystalline MCM-41. When the incubating time is less than 30 min, only amorphous phase is obtained after the thermal treatment, and after 2 hours of incubation, reasonably crystalline MCM-41 (denoted MCM-41-F) forms upon thermal treatment. The XRD spectra show that the gel at room temperature is highly amorphous since there is no diffraction peak on its XRD pattern whereas the sample calcined at 550 ~ exhibits some crystallinity as suggested by the diffraction peak at around 1.7 ~ corresponding to a d-spacing
MCM-41-A
/
600 MCM-41-A
MCM-41-B
400
200
MCM-41-F
MCM-41-F !
10 20 PORE DIAMETER, nm
Fig. 3 The pore distribution curves of MCM-41-AI, D1 and FI
0
0.2 0.4 0.6 0.8 RELA'FIVE PRESSURE, p/p, Fig. 4 The N2-adsorption isotherms of MCM-41 -A 1, B2 and F 1
1.0
82 of 50 A. The pore size distribution based on the desorption branch reveals that there are two mesopores sizes in the products (Fig. 3): one with an average pore diameter of about 30 A, the other
within the range 80-200 A. The majority of mesopores are within the range
between 80-200 A and the maximum of the distribution curve is at around 110 A. It is believed that these large mesopores are similar to those present in amorphous mesoporous silica gels, being formed by the packing of small silica particles. The total pore volume for narrow pores (30 A) is only 0.12 cm 3gl corresponding to a total surface area of 150 m/g -l, whereas that for the large pores (110 A) is 1.35 cm3g-1 with a total surface area of 430 m 2 g~. From the N2-adsorption isotherms for MCM-41 materials (Figure 4), we can see that the pore regularity of MCM-41-FI is less than that of MCM-4 l-A1 and B2 [11]. The Na20/SiO2 ratio in the gel affects to a great extent the appearance of the XRD patterns of the precursor and the calcined samples. For instance, with Na20/SiO2>0.25 leads to a gel precursor with XRD pattern showing clearly a peak between 1~ and 2 ~ Whereas with Na20/SiO2<0.12, no diffraction peak appears at all. Figure 5 shows the SEM graphs of three typical MCM-41 samples selected from Table 1. The particle size of the sample prepared at room temperature (MCM-41-D1) is about 20~tm whereas those for MCM-41-A1, B2, C1, and E1 are between 0.1 and 0.3 lam. It seems that low temperatures favor the formation of relatively large particles.
MCM-41-B2 samples
possess lower BET surface areas, larger pore volumes and pore sizes compared with MCM41-A1 and D1 samples. The pore size of MCM-41-D1 is exceptionally small (about 20 A). Both MCM-41-AI and D1 were prepared from gels with higher H20/SIO2 ratios. Therefore, it is believed that the H20 content in the reaction mixture plays an important role in determining the pore features of the product. MCM-41-D 1 and E 1 have a pore distribution
Fig. 5 The SEM micrographs of MCM-41-A I, B2 and D l
83
as-synthesized
/
calcined calcined
I
200
J
l
I
100
,
I
0 8, ppm
I
9
-100
, .
100
0
-100
-200
-300
8, ppm
Fig.6 27A1MAS NMR spectra of MCM-41-A1 Fig.7 29Si MAS NMR spectra of MCM-41-A1 similar to that for MCM-41-A1. The 27A1 MAS NMR spectra of the as-synthesized and calcined Al-containing MCM-41-A1 sample is shown in Fig. 6. The signal at -51 ppm is attributed to tetrahedrally coordinated AI, and it is seen that only tetrahedral AI is present in the as-synthesized material. Upon calcination, a small amount of octahedrally-coordinated AI was formed which corresponds to the weak signal at about 0 ppm. It is quite likely that during calcination, a part of the tetrahedrally-coordinated framework AI atoms move outside to the extraframework positions where they become 6-coordinated. The 29Si MAS NMR spectra (Fig. 7) indicates that Q3(Si(O)3(OH)) and Q4(Si(O)4) species exist in both assynthesized and calcined MCM-41-A1 sample. After calcination, however, a signal (-91 ppm) corresponding to Q2(Si(O)2(OH)2) species appears clearly, suggesting that the removal of the template molecules increases the amount of the Si-OH groups in the structure. 4. CONCLUSIONS Under hydrothermal preparative conditions, reaction gels with a H20/SIO2>80 give rise to MCM-41 materials possessing high surface areas and small pore sizes. Whereas that with 1-110/SIO2<80 the products possess lower surface areas and larger pore sizes. New routes including direct thermal treatment, room-temperature crystallization and microwave heating were developed for synthesizing the mesoporous MCM-41. With appropriate gel
84 compositions, MCM-41 materials crystallize at room temperature or under microwave treatment. Direct thermal treatment of certain wet gels at an elevated temperature (550~ also leads to cr3stalline MCM-41 materials. The products possess a bimodal mesopores distribution: one is about 30 A and the large one within 80-200 fi, Some solid samples recovered from hydrothermally treated gels are XRD-amorphous, but as used as precursors for thermal treatment they transform to MCM-41 molecular sieves. In contrast to hydrothermal synthesis, these new routes exhibited obvious features in the following: very short time, very simple, and selective formation of the pore size. MAS NMR spectroscopy reveals that after calcination a small part of the tetrahedraily-coordinated framework aluminum atoms becomes octahedrally-coordinated and a considerable amount of Si-OH species is generated. ACKNOWLEDGMENT We are grateful to the National Natural Science Foundation of China, the National Doctoral Science Foundation of China, and the KeyLaboratory of Inorganic Hydrothermal Synthesis of Jilin University for financial support. REFERENCES
[1]C.T. Kresge, M.E. Leonowicz, W.J. Roth, and J.S. Beck, Nature, 359 (1992), 710 [2]J.S. Beck, J.C. Vartuli, W.J. Roth, et al., J. Am. Chem. Sot., 114 (1992), 10834 [3]J.S. Beck, C.T. Chu, et al., US Patent No. 5 108 725 [4]C.Y. Chen, H. Li, M.E. Davis, Microporous Materials, 2 (1993), 17 [5]Q, Huo, D.I. Margolese, U. Ciesla, et al., Nature, 368 (1994), 317 [6]A. Monnier, F. Schuth, Q. Huo, et al., Science, 261 (1993), 1299 [7]V. Aifredsson, M. Keung, A. Monnier, G. Stucky, J.C.S. Chem. Commun., 921 (1994) [8]A. Steel, S.W. Carr and M.W. Anderson, J.C.S., Chem. Commun., 1571 (1994) [9]P.T. Tanev, M. Chibwe and T.J. Pinnavaia, Nature, 368 (1994), 321 [10]P. Chu, F.G. Dwyer, J.C. Varfull, Eur. Patent Appl., 358 (1990), 827 [1 I]R. Schmidt, M. Stocker, E. Hansen, Microporous Mater., 3 (1995), 443
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
85
Synthesis and characterization of FeSiMCM-41 and LaSiMCM-41 Nong-Yue He, Shu-Lin Bao and Qin-Hua Xu* Department of Chemistry, Nanjing University, Nanjing 210093, P.R.China Mesoporous materials SiMCM-41, FeSiMCM-41, LaSiMCM-41, A1SiMCM-41, and La~SiMCM-41 were synthesized. The mesoporous structure of these materials was characterized by XRD, FT-IR, nitrogen and benzene adsorption methods. EPR and Mossbauer spectra suggested the incorporation of Fe(III) in the channel wall of -synthesized FeSiMCM41 sample. The introduction of Fe(IIl) and La([II) inproved the thermal and hydrothennal stabilities of SiMCM-41. I. INTRODUCTION The synthesis of mesoporous materials with the regular array of uniform, One-dimensional mesopore in the range of - 1.5 to greater than 10 nm designated MCM-41 by the Mobil researchers is widely interesting[ I-9]. One of interested objects is to improve its hydrothermal stability[ 10-12]. It was well known that ferric and rare earth elements play an important role in modifying zeolite molecular sieves. However, though the lamellar or unidentified iron oxide mesostructured materials have been reported [5,7] and a Fe-containing MCM-41 mesoporous molecular sieve with SiO2/Fe203 molar ratio 150 using fumed silica as silica source has been reported too[13], the hexagonal FeSiMCM-41 has not yet been studied in detail In the present study, we detailly discussed the synthesis and characterization of FeSiMCM-41 and LaSiMCM-41, and investigated their thermal and hydrothertmal stabilities. 2. EXPERIMENTAL The FeSiMCM-41 mesoporous materials with different SiO2/Fe203 ratio were prepared according to the following synthesis procedures: 11 g distilled water, 0.4 g sulphuric acid(95%), and optionally, different ammounts ofFe(NO3)3 - 9H20, varying from 0 to 0.71 g, were mixed and stirred for 10 rain. Then 8.6 g sodium silicate (20.3%SIO2, 6.7%Na20) were added. After stirring the formed mixture for 10 rain, the appropriate ammotmt template solution(25% CTABr) was added. The formed gel was stirred for 30 rain before adding 6.7 g distilled water. Then the gel was transfered into a stopped teflon-lined steel bottle and heated without stirring at 373K for 7 or 14 days. After cooling to room temperature, the resulting solid product was recovered by filtration, extensively washed with distilled water, and dried in air at ambient temperature. The colour of the as-synthesized FeSiMCM-41 from gel mixture with SiO2/Fe203 ratio from 67 to 133 was white, but the color of as-synthesized FeSiMCM-41 sample from the gel mixture with SiO2/Fe203 ratio 33 was pale yellow. The preparation of LaSiMCM-41 mesoporous materials was similar to that mentioned above except for substituting lanthanum
86 nitrate for ferric nitrate. For comparison, AISiMCM-41 samples were also synthesized by means of adding a given ammount of sodium aluminate into the g d mixture instead of fenic nitrate. The dried products was calcined at 813 K in flowing nitrogen followed by air for 4h to remove the template. The calcined samples were characterized by low-angle X-ray powder diffraction (Rigaku,D/max-rA) with Cu-K cx radiation, FT-IR(Nicolet, 5DX), EPR (Bruker EP 200-DSRC), the Mossbauer spectrum (recorded on a constant acceleration Mossbauer spectrometer with a source of 57Co in Pd matrix), the adsorption of nitrogen at 77K (Micromeritics, ASAP2400 instrument) and benzene adsorption at 298 K (on an conventional gravimetfic method). To compare the thermal stability, the above calcined samples were calcined once more in a muft]e stove in air at 1153 K for 2 h respectively, followed by XRD detection. The composition of ~mples were obtained on a Jarrell-Ash 1100 inductively coupled plasma quantometer. The hydrothermal stability of samples treated with 100% steam at 933 K for 2 h were investigated by benzene adsorption technique. 3. RESULTS AND DISCUSSION 3.1 XRD The powder X-ray di~action patterns of calcined samples are shown in Figure 1. q]~e observation of four peaks of samples which can be indexed on a hexagonal lattice is typical of MCM-41 materials[I]. Owing to the lack of good long-range hexagonal order[3], the (110) and (200) peaks of sample 8 overlapped each other. Table 1 The composition of gel mixtures and samples* Molar composition of.the gel Sample CTAB SiO2 A1203 Fe203 La203 Na20 H20 1 2 3 4 5 6 7 8 9
0.25 0.25 0.25 0.25 0.25 0.25 0.25 0.25 0.25
1 0.18 1 0.008 0.18 1 0.015 0.18 1 0.030 0.18 1 0.008 0.18 1 0.015 0.18 1 0.030 0.18 1 0.015 0.015 0.18 1 0.015 0.18
57 57 57 57 57 57 57 57 57
As-synthes~ed samples SiO2/m1203 SiO2/Fe203 SiO2/La203 pure siliceous 124 62 32
40 58
147 83 48 116
* Crystalized at 373 Kfor 7 days(samples 1 and 9) and 14 days (samples 2-8). The hexagonal FeSiMCM-41 and LaSiMCM-41 mesoporous molecular sieves were synthesized from the given gel mixtures as shown in Table l.The white color of as-synthesized
87 samples 2 and 3 exln'bites the absence of coloured oxides of iron and may give an indication of Fe(IlI ) incorporated into the framework position.
I
a a
b
b C
d e
2
4
6
8
2 | (degrees) Figure 1 XRD patterns of calcined samples a--sample 1, b--sample 3, c--sample 6, d--sample 8, e--sample 9
Figure 2 EPR spectra of as-synthesized samples FeSiMCM-41 samples. a--sample 2, b--sample 3, c--sample 4
The d-spacing and lattice parameters of samples are listed in Table 2, it is shown that the dl0o and the lattice parameter of calcined MeSiMCM-4 I(Me=AI, Fe and La) are greater than those of SiMCM-41, consistent with the Me-O bonds longer than Si-O bond and giving an evidence of Me(III) incorporation into framework position too. Table 2 Characterization of samples Before calcination Sample dloo a (nm) (nm) 1 3 6 8 9
4.27
4.93
4.29
4.95
* Lattice parameter a=dlo02v/3.
After calcination d~0o a (nm) (nm) 4.03 4.46 4.08 4.19 4.15
4.65 5.15 4.71 4.84 4.79
pore size (BJl-Lnm) 3.2 3.3 3.3 3.0 3.3
surface area (m2/g) 1340 947 932 944 1084
88 3.2 EPR spectra
The EPR spectra ofFeSiMCM-41 ~mples containing different SiO2/Fe203 ratio are shov~n in Figure 2. There are two signals in all the spectra, g--4.3 and g=2.0, assigned to tetrahedrally and octahedraUy coordinated Fe(Ill) respectively[14]. We found the relative intensity of sig~lal with g=4.3 to that of g=2.0 decreased with the increase of Fe(III) content in FeSiMCM-41 samples. Therefore, the amount of Fe( III ) incorporated into the framework position was limited. 3.3 Mossbauer Spectra
The Mossbauer spectra of sample 3 are shown in Figure 3a. The isomer shift (IS) of assynthesized sample is 0.28 mm/s, correspondent with tetrahedrally coordinated Fe( [II ) in framework[15]. Therefore, Fe(III) was mainly incorporated in fxamework positions of assynthesized FeSiMCM-41 sample. However, after calcination at 813 K for 4 h in air, The isomer ~ifl increases to 0.43 ram/s, which was ascribed to octahedrally coordinated Fe(I!!) (Figure 3b). It meant that the tetrahedrally coordinated Fe(III) had been mostly transformed to octahedrally coordinated Fe(Ill). This result is consistent with the EPR data of calcined samples(see Figure 7c). a
/b ~
.. '. :: ~" :.-. ~
a
--~........r C
Z
J
o
" " " ."
~'.'..X':
-)(..':'"."
"''"
fd
9
te
o
O
-.,.~'~
.,.
.... :, .. ~.?~.. ".. I
-5.0
-2.5
9:
.o
~?..
."
.~'...~.."':':. ~"
|
t
0.0
2.5
5.0
__t
1200
1000
800
600
400
VELOCITY (mm/s) WAVENUMBERS (cm-~) Figure 3 Mossbauer spectra of sample 3. (a)--as-synthesized (b)--after calcination at 813 K for 4 h in air
Figure 4 FT-IR spectra for calcined samples and fumed silica. a--sample 1, b--sample 3, c--sample 6, d--sample 9, e--fumed silica
3.4 F r - I R
FT-IR spectra of samples 1,3,6,and 9 are similar to the amorphous fumed silica (Figure 4), therefore, the channel wall of the as-synthesized mesostructured materials is amorphous[2l Compared with the spectrum of SiMCM-41, all the bands of MeSiMCM-41 (Me=Fe, La and
89 AI) shift to lower wavenumbers, indicating Fe(III), La(III) and Al(IlI) may be incorporated into the chaired wall, for Me-O bonds are longer than Si-O bond.
3.5 Adsorption experimentais Figure 5 shows the nitrogen adsorption-desorption isotherms for the samples at 77 K. All the isotherms exhibit a sharp inflection at a relative pressure about 0.36 characteristic of capillary condensation with uniform mesopores. The BJH pore size distribution indicates a narrow pore size distribution for all the samples at about 3.0-3.3 nm (see Table 2).
700
b
900
500
400
100
100
f I
I
0.2
0.4
I
0.6
I
rl
0.8
1.0
700
0
,,,
0.2
_1
i I
0.4
0.6
. I
0.8
1.0
900 C
d
400
500 f
100
100 4
!
0.2
0.4
I
0.6
i
0.8
900
1.0
0
0.2
i
0.4
e
r~
500
100 r
I
0.2
0.4
0.6
0.8
P/Po Figure 5 Adsorption isotherems of nitrogen of calcined samples. a--sample 1, b--sample 3, c--sample 6, d--sample 8, e--sample 9
1.0
,
i.
I
0.6
0.8
1.0
90 The BET surface area are also given in Table 2. Compared with the pure siliceous sample, the surface area of samples containing Fe, La and AI decreases slightly. 3.6 Thermal and hydrothermal stabilities It was noted that the (100) peak intensity of XRD for the template-removed SiMCM-4 I was very strong before calcination at 1153 K (Figure 6(a)), but it become weaker after the calcination with a decrease of d-spacing about 0.33 nm Conversely, the peak intensity of FeSiMCM-41(sample 3) was decreased slightly and the d-spacing only changed 0.05 mn after the same calcination (Fig.6(b)), while A1SiMCM-41 lost most of its structure after the calcinmation. Then compared samples calcined in air with that in N2 followed by air, the XRI) patterns ofFeSiMCM-41 and LaSiMCM-41 made no significant changes, while the (100) peak intensity of AISiMCM-41 decreased obviously, which suggested the incorporation of AI decreased the thermal stability of SiMCM-41. DTA curves for samples showed that FeSiMCM-41, LaSiMCM-41, SiMCM-41 and AISiMCM-41 collapsed starting at 1163, I 160, 1153 and 1149 K respectively. Thus, the order of thermal stability of samples obtained fi'o~n XRD and DTA data is shown as following: FeSiMCM-41 = LaSiMCM-41 > SiMCM-41 "; A1SiMCM-41.
e ~
.ill~,
"" i
l..,, IJ
__
i
2
4
6
2 | (degrees)
8
2
4
6
8
2 | (.degrees)
Figure 6 The XRD patterns for calcined (a) sample 1 and (b) sample 3, solid lines befbre calcination, dashed lines after calcination at 1153 K in air for 2 h. It was reported that the framework of A1SiMCM-41 collapsed at 963 K in stea~n treatmemt[3]. In our study, AISiMCM-41 (sample 9) steamed at 933 K lost its XRD pattten~ almost completely, which indicated its poor hydrothermal stability. However, FeSiMCM41(sample 3) and LaSiMCM-41(sample 6) still remained a stronger (100) peak and a high equih'bdum adsorption capacity for benzene under the same treatment conditions. Compared XRD values of Ill0 and c/c0 listed in Table 3, the sequence of the hydrothermal stability of samples is, FeSiMCM-41 = LaSiMCM-41 > SiMCM-41 > LaSiMCM-41 > AISiMCM-4 I.
91 From the above results, we suggest that the introdoction of Fe or La into the SiMCM-4 I increase both the thermal and hydrothermal stab'dities, while AI decrease them. Table 3 Hydrotherm__al stability of samples Before steam treatment
Sample
d,oo(nm)
1 3 6 8 9
4.03 4.46 4.08 4.19 4.15
After steam treatment
co(g/g)
dl0o(llm)
0.680 0.605 0.548 0.465 0.655
3.72 4.12 3.72
c(g/g) 0.381 0.408 0.348 0.234 0.278
1/I0(%) 54 81 83 very weak peak very weak peak
c/c0(%) 56 67 64 50 42
I0, I : The intensities of(100) peaks before and after steam treatment respectively. co, c : The adsorption capacity for benzene at P/P0=0.5 before and after steam treatment respectively. Figure 7 shows the EPR spectra ofFeSiMCM-41 at different calcination time. It was found that the color of FeSiMCM-41 samples changed from white to brown by increasing the calcination time, accompanied by decreasing the signal intensity at g=4.3 and increasing that at g=2.0 (Figure 7 b-d), suggesting that the tetrahedrally coordinated Fe(III) in as-synthesized sample FeSiMCM-41 progressively converted to octahedrally coordinated Fe(Ill) as hmreashlg the calcination time. The Mossbauer spectra also shows the same change of the coordination
8 a
b
d
Figure 7 EPR spectra of calcined sample 3. a--as-synthesized, b--1 h, c--4 h, do-8 h calcined at 813 K in air
92 enviroment of Fe(III) before and after the calcination (Figure 3). Thus, we suggest that the octahedrally coordinated Fe( Ill ) species in FeSiMCM-41 may increase the thermal and hydrothermal stabilities of the channel wall ofmesoporous material 4. CONCLUSION The hexagonal mesoporous FeSiMCM-41 and LaSiMCM-41 have been synthesized using sodium silicate as silica source. Fe( III ) and La( III ) species may impove the thermal and hydrothermal stabilities of SiMCM-41 but AI(III) destabilizes it. It seems that octahedrally coordinated Fe(Ill) species led to increase of thermal and hydrothermal stabilities of the channel wall ofmesoporous FeSiMCM-41. REFERENCES
1. C.T.Kresge, M.E. Leonowicz, W.J.Roth, J.C.Vartuli and J.S.Beck, Nature, 359 (1902) 710. 2. J.S.Beck, J.C.Vartuli, W.J.Roth, M.E.Leonowicz, C.T. Kresge, K.D.Schmitt, C. T-U. Chu, D.H.Olson, E.W.Sheppard, S.B. McCullen, J.B.Higgins and J.L.Schlenker, J.Am. Chem Soc., 114(1992) 10834. 3. A.Monnier, F.Schuth, Q. Huo, D. Kumar, D. Margolese, R.S. Maxwell, G.D. Stucky, M. Kishnamurthy, P. Petroff, A.Firouzi, M. Janicke and B. F. Chmelka, Science, 261 (1993) 1299. 4. C.Y. Chen, S.L. Burkett, H. X. Li and M. E. Davis, Microporous Materials, 2 ( 19q3 ) 27. 5. Q. Huo, D.I. Margolese, U. Ciesia, P. Feng, T.E. Gler, P. Sieger, IL Leon, P. M. Petroft~ F. Schuth, and G. D. Stucky, Na~-~, 368 (1994) 317. 6. P. T. Tanev, M. Chibwe and T. J. Pinnavala, Nature,368 (1994) 331. 7. P. L. Llewellyn, U. Ciesla, H. Decher, R. Stadler, F. Schuth and K.K. Linger, Stud. Surt~ Sci. Catal., 84 (1994) 2013. 8. A. Corma, M. T. Navarro, J. Perez-Pariente and F. Sanchez, Stud. Sure Sci. Catal., 84 (1994) 69. 9. O. Franke, J. Rathousky, G. Schulz-Ekloff~ J. Starek and A. Zukal, Stud. Surf Sci. Catal.. 84 (1994) 77. 10. S.B.McCullen, J.C. Vartttli and W. Chester, Method for Stabili~ng Synthetic Mesoporous Crystalline Material, U.S Patent No. 5 516 829(1992). 11. N. Coustel, F. Di Renzo and F. Fajula, J. Chem. Sot., Chem. Commun., (1994) 967. 12. R. Ryoo andJ. M. Kim, J. Chem. Sot., Chem. Commtm., (1995) 711. 13. Z.Y. Yuan, S.Q.Liu, T. I-L Chen, J.Z. Wang and H.X. Li, J.Chem.Soc., Chem. Commum.. (1995) 973. 14. 1LSzostak, V.Nair and T.L.Thomas, J.Chem.Soc.Faraday Trans.I.(1987) 487. 15. P. Ratnasamy and 1L Kumar, Catal. Today, 9 (1991) 329.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
93
Synthesis of titanium-containing mesoporous molecular sieves with a cubic structure K. A. Koyano and T. Tatsumi Engineering Research Institute, Faculty of Engineering, The University of Tokyo, Yayoi, Tokyo 113, Japan 1. INTRODUCTION Recently a new family of mesoporous molecular sieves named M41S was discovered by the researchers at Mobil [1, 2]. The M41S family is classified into several members: MCM-41 (hexagonal), MCM-48 (cubic) and other species. These materials have uniform pore, and the pore size are able to be tailored in the range 16/~ to 100/~ through the choice of surfactant, auxiliary chemicals and reaction conditions. Because of the favorable uniformity and size of the pore, synthesis and utilization of mesoporous materials have been investigated by numbers of researchers. Some circumstantial reports about the synthesis have been made [3-5]. Adsorption property and catalytic activity of silica-based and Al-containing MCM-41 have also been reported [6, 7]. Ti-, V-, B-, Fe- and Mn-substituted MCM-41 and Ti-substituted hexagonal mesoporous silica (Ti-HMS) have also been synthesized [8-15]. These Ti- and V-substituted mesoporous molecular sieves pioneered the potential to oxidize bulky molecules which cannot enter into the micropores of zeolites such as TS-1, TS-2 and Ti-beta. MCM-48, characterized by a three-dimensional channel system, may have several advantages over MCM-41 with a one-dimensional channel system when applied to catalytic reactions: for instance, the three-dimensional pore system should be more resistant to blockage by extraneous materials than the one-dimensional pore system. Here we report the synthesis of Ti-MCM-48 and its use as a catalyst for epoxidation of alkenes and unsaturated alcohols. The effects of gel composition and the gel preparation method on the structure of mesoporous materials are also reported. 2. EXPERIMENTAL
Mesoporous materials were synthesized under hydrothermal conditions at 373 K in a static Teflon bottle for 10 days. The procedures of gel preparation were as follows. For the preparation of pure silica mesoporous materials, an aqueous solution of cetyltrimethylammonium chloride / hydroxide (CTMACI/OH, CI/OH - 70/30) was added dropwise to tetraethyl orthosilicate (TEOS) under vigorous stirring at 278 K. After stirred for 1 h, the mixture was heated at 358 K for 4 h to remove the ethanol produced in the hydrolysis of TEOS. For the synthesis of Ti-containing mesoporous materials, two types of hydrolysis method were employed. Ti-MCM-48(1) was prepared by a one-stage hydrolysis method: TEOS and tetrabutyl orthotitanate (TBOT) were hydrolyzed simultaneously after being mixed for 30 minutes at 298 K. Ti-MCM-48(2) was prepared by a two-stage method : To a 44% solution
94 of TEOS in propan-2-ol, CTMAOH in methanol and water (water / TEOS (molar) = 2) were added to partly hydrolyze TEOS at 278 K. After 1 h, a propan-2-ol solution of TBOT was added to this resultant mixture very slowly under vigorous stirring. The.mixture was then stirred for 1 h, when the aqueous solution of CTMAC1 was finally added. When water-glass (SiO 2 = 28 - 30%, Na20 = 9 - 10%) was used as the Si source, sulfuric acid was added to the mixture in order to adjust the pH to 11.6 and CTMAC1 was used as the template. The molar compositions of the gels subjected to hydrothermal synthesis (373 K, 10 days) were as follows : SiO 2. xTiO 2 9yNa20 9CTMA 9zH20, where 0 _< x _<0.02, y = 0 (TEOS) or 0.29 0.35 (water-glass), and 46.5 _
3. RESULTS AND DISCUSSION 3.1. Time course of hydrothermal synthesis Before we attempt to introduce Ti into the framework of MCM-48, we investigated the optimal conditions for the synthesis of pure silica MCM-48. Since it was found that the incorporation of titanium into zeolite frameworks was negatively affected by the presence of alkali cations, TEOS was used as the Si source. In the preparation of MCM-48, we conducted the hydrothermal synthesis in a Teflon
(211)
(420) .,..~ r~
(c) (B)
(A) 2
4
6
20 / degree
8
10
Figure 1. Change of XRD pattern with time in hydrothermal synthesis of MCM-48. (A) 2.5 days, (B) 6 days, (C) 10 days.
95 bottle at 373 K after keeping the mother liquids at 358 K for 4 hours to remove alcohols. The composition of reaction mixture was TEOS / CTMA / H20 = 1 / 1 / 46.5. As shown in Figure 1, mesoporous structure was formed after 2.5-day hydrothermal treatment. The typical pattern of the cubic structure with one strong peak and 7 weak ones in the 20 range of 2-7 ~ distinctly appeared after 10 days. This finding indicates that 10-day hydrothermal treatment is required to synthesize MCM-48 with the cubic structure, using TEOS as the Si source under our conditions. It is to be noted for the synthesis of MCM-41 under the same hydrothermal conditions except for the composition of reaction mixture ( TEOS / dodecyltrimethylammonium (DTMA) / H20 = 0.75 / 1 / 84 ), the formation of hexagonal structure also required 10 days while mesoporous structure was formed before the hydrothermal treatment. 3.2. Effect of surfactant concentration
Vartuli et al. have reported that the surfactant/silica molar ratio (Surf/Si) is a critical variable in the formation of M41S materials; cubic mesoporous material MCM-48 was formed when the Surf/Si ratio was adjusted to 1-1.5 [5]. We attempted the synthesis of mesoporous materials by varying the concentration of the surfactant with the Surf/Si ratio kept constant at 1.0. At 20.0 wt% of CTMAC1/OH (70/30) (H20/CTMA = 69.8), MCM-41 was exclusively obtained. The structure was transformed from hexagonal into cubic with increasing concentration of the surfactant (Table 1), in good agreement with the effect of concentration on the formation of a liquid-crystal phase for the CTMA system [16]; the cubic phase is favored over the hexagonal phase at higher concentrations for the chloride containing system. Obviously, the structure of the products was affected not only by Surf/Si but also by the surfactant concentration. Using TBOT as the Ti source, Ti-MCM-48-(1) and -(2) molecular sieves were successfully obtained from the gels with the following molar compositions: SiO 2 9 0.01TiO 2 90.7CTMACI 90.3CTMAOH 946.5I-I20. The increase in the Ti content to Si/Ti = 50 (two stage hydrolysis method) resulted in the formation of an ill-defined mesoporous material, which showed only one strong intensity peak at ca. 20 = 2 o. Table 1 Effect of concentration of surfactant and Si source on the structure of products Si source a
Si/Ti b
TEOS TEOS TEOS TEOS
0 0 100 50
H20/CTMA 69.8 c 46.5 c 46.5 c 46.Y
structure hexagonal cubic cubic ill-defined mesoporous
aTEOS: tetraethyl orthosilicate, Si/CTMA (cetyltrimethylammonium) = 1.0. bTi source : tetrabutyl orthotitanate, c CTMAC1/OH = 70/30. Hydrothermal synthesis conditions: 373 K; 10 days; under static condition. 3.3. Effect of Si source
Using colloidal silica as a Si source instead of TEOS, MCM-48 was obtained; however, the crystallinity was slightly lower than the product formed from TEOS. (Figure 2) When water-glass was used as the Si source, MCM-41 was obtained from the gels with the same Surf/Si and HzO/Surf ratios from which MCM-48 was obtained. There is an important
96
,i..o
(c) O
/
/
(A) !
0
2
4 6 20 ! degree
8
10
Figure 2. XRD patterns of as-synthesized mesoporous materials prepared from various Si sources. (A) TEOS, (B) colloidal silica, (C) sodium silicate.
difference between the Si sources; water-glass giving MCM-41 contains a large amount of Na, in contrast to TEOS and colloidal silica which give MCM-48. When a small amount of Na § (Na/Si molar ratio = 0.15) was added to TEOS together with the surfactant, the ill-defined mesostructure was formed. Even when Na § was added to the gel prepared from TEOS immediately before the hydrothermal treatment, we obtained poorly crystalline material. It has been shown that the addition of Na § dramatically changes the phase diagram of aqueous CTMA [ 17]. Thus it is conceivable that the presence of Na seriously affected the structure of the products. The details will be reported elsewhere. 3.4. Effect of pH
The pH is one of the important factors in the synthesis of all the kind of zeolites. We investigated the effect of pH by varying the ratio of anion of surfactant (CTMAC1/OH 70/30, 80/20, 90/10). As shown in Figure 3, the cubic structure was formed at the CTMAC1/OH = 70/30. With decreasing pH, the product structure was transformed from cubic into ill-defined
d .,..~ r~
(c)
O
(B) ~ ,-"-7~--4
,,
,(A)
6
8
20 / degree
Figure 3. XRD pattems of as-synthesized mesoporous materials prepared by variety of CTMACI/OH ratios. (A) 90/10, (B) 80/20, (C) 70/30.
97 mesostructure and finally amorphous. No solid products were obtained at the pH higher than 12. These results lead to the conclusion that the appropriate pH for the synthesis of MCM-48 is the range of 11 - 12.
3.5. Ti-eontaining MCM-4$ Titanium-containing mesoporous material with the cubic structure, Ti-MCM-48, has been synthesized by the addition of tetrabutyl orthotitanate as a Ti source. As shown in Figure 4, Ti-MCM-48(1) exhibited a very strong peak at d - 35.6 A and medium or weak peaks a t d = 31.0, 23.4, 21.8, 19.5, 18.6, 17.9 and 17.2/~. These eight peaks were indexed on a cubic unit cell with a - 87.2/~. The nitrogen physisorption isotherm was characteristic of mesoporous materials with uniform pore size. The average pore diameter determined by the Dolimore-Heal method was 25/~ and the BET surface area was ca. 1000 m2g1 . These data totally agree with those of pure silica MCM-48. We studied the pore structure of Ti-MCM-48 by high resolution transmission electron microscopy. Figure 5 exhibits a monoclinic type repeat pattern containing a 109.5 ~ angle, on the cubic [110] phase. Besides, typical regular two-dimensional patterns, such as [111] and [100], were observed, although most of the observed sheets show [111] or [110] patterns. These observations were in good agreement with those made by Mobil researchers for pure-silica MCM-48 [5]. From the XRD and TEM patterns, it has been revealed that the symmetry of Ti-MCM-48 was consistent with an I a 3 d space group, as was proposed by Schmidt et al. [18]. No differences in the TEM patterns were found between pure silica MCM-48 and Ti-MCM-48. As shown in Figure 6, solid-state 29Si MAS NMR spectrum of Ti-MCM-48 closely resemble that of pure silica MCM-48. These spectra are able to be separated into three broad peaks from Q4, Q3 and Q2 silicones by an appropriate choice of CP conditions. Though the peaks were rather broad, Q3 content (27%) roughly agreed with the N/Si molar ratio (= 0.30) observed for the as-synthesized pure silica materials [5]. This agreement in absolute numbers, .
.
.
.
.
.
.:
..
.. . . . . . .
...
..
:,::
,..
:...
:
.
.
.
.
.
r~
.~
(B___2____) (A) I
0
2
I
I
4
6
I
8
10
-'~-- bU n m ~
.t ~ .~:, ~. - %~ . - %m ~.m-. ~' m. . . - 9~
20 / degree
Figure 4. XRD patterns of MCM-41. (A) pure silica MCM-48, (B) Ti-MCM-48(1)
Figure 5. Transmission electron micrographs of Ti-MCM-48(1) showing the [110] projection.
98 Q3 (27%) and the N/Si ratio (30%) may indicate that Q3 is associated with the surfactant. The UV-VIS spectra for the Ti-MCM-48 samples are shown in Figure 7. The band at 220 nm has been assigned to isolated framework titanium in tetrahedral coordination [19]. TiMCM-48(1) showed a broad shoulder at ca. 270 nm attributed to extraframework titanium [20]. The anatase band, which occurs at 312 nm, seems to be superimposed on this band. In contrast, Ti-MCM-48(2) proved to be essentially free of extraframework titanium. These results indicate that the two-stage hydrolysis method is favorable for the isomorphous substitution of Ti for Si. This is interpreted in terms of the prerequisite condition to the efficient incorporation of Ti in the zeolite framework observed for TS-I: the rate of hydrolysis of Ti alkoxide should match that of Si alkoxide [21 ].
3
(B) (A) ! . . . . . . .
. . . . .
. . . .
. . . .
'-14o
ppm from TMS Figure 6. 29Si MAS NMR spectra of MCM-48. (A) pure silica MCM-48, (B) Ti-MCM-48(1).
200
!
400 600 Wavelength / nm
800
Figure 7. UV-VIS spectra of Ti-MCM-48. (A) Ti-MCM-48(2), (B) Ti-MCM-48(1).
3.6. Catalytic activity The oxidation of cyclododecene (c&/trans = 75/25) was performed using Ti-MCM-48, Ti-MCM-41, TS-1 and amorphous TiO2-SiO 2 with H202 or TBHP as the oxidant at 323 K. Ti-MCM-41 was synthesized at Surf/Si = 0.6, H20/CTMA = 75, and Si/Ti = 80 by the two stage method. As shown in Table 2, cyclododecene was epoxidized to cyclododecene oxide with either TBHP or H202 on Ti-MCM-48 and Ti-MCM-41. Preference for the epoxidation of trans-isomer was obtained for both oxidants. No other products were detected. The high activity of Ti-MCM-48 materials compared to Ti-MCM-41 may be due to the three-dimensional pore structure of Ti-MCM-48; Ti-MCM-48(2) was slightly more active than Ti-MCM-48(1). Amorphous TiO2-SiO 2 showed a very low activity in the epoxidation using H202. Compared with Ti-MCM-48(1), TiO2-SiO 2 showed a much more substantial difference in activity with H20 2 and TBHP, probably owing to severe inhibition of the catalyst by water [22]. No products were obtained with TS-1 probably as a consequence of the inability of cyclododecene to diffuse into the pores of TS-1 (5.6 x 5.3/~). Ti-MCM-48 was also applicable for the epoxidation of other alkenes. In the oxidation of pent-2-en-l-ol (10 mmol) using Ti-MCM-48(2) (100 mg) with H20 2 (60 mmol), oxidation
99 products were obtained in 17% yield (turnover number: 95); selectivities for epoxidation of the double bond and oxidation of the alcoholic group to aldehyde were 46 and 54%, respectively. The high reactivity of pent-2-en-l-ol compared to cyclododecene may be ascribed to the enhancement effect of the OH group [23]. Table 2 Epoxidation of cyclododecene on titanium-containing materials
Catalyst Ti-MCM-41(2) Ti-MCM-48(1) Ti-MCM-48(2) TS-1 TiO2-SiO 2
Si/Ti 71 80 83 79 85
Turnover Number (mol/mol-Ti) Oxidant H20 2 TBHP 0.73 (54/46)" 1.50 (59/41) ~ 1.61 (58/42)" 0 0.057 (-)"
--7.1(34/66)" --m 2.6 (30/70)"
"cis/trans ratio of products. Reaction conditions: 50 mg catalyst; 20 mmol cyclododecene (cis/trans = 75/25); 24 mmol oxidant; 323 K; 2 h. 4. CONCLUSION Titanium-containing mesoporous material with a cubic structure, Ti-MCM-48, has been successfully synthesized by means of using tetraethyl orthosilicate as a Si source under appropriate reaction conditions. Ti-MCM-48 has been found to show activity for epoxidation of bulky alkenes with H202. as well as tert-butyl hydroperoxide as an oxidant. The high catalytic activity of Ti-MCM-48 compared to Ti-MCM-41 may be related to its threedimensional channel system. 5. A C K N O W L E D G E M E N T S
The authors are grateful to Prof. S. Namba (The Nishi-Tokyo University) for measuring high resolution transmission electron micrographs, and also wish to thank Dr. S. Nakata (Chiyoda Corporation) for measuring 298i MAS NMR spectra. REFERENCES
1.
C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli and J.S. Beck, Nature, 359
2.
J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T-U. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins and J.L. Schlenker, J. Am. Chem. Soc., 114 (1992) 10834. J.S. Beck, J.C. Vartuli, G.J. Kennedy, C.T. Kresge, W.J. Roth and S.E. Schramm,Chem. Mater., 6 (1994) 1816. J.C. Vartuli, C.T. Kresge, M.E. Leonowicz, A.S. Chu, S.B. McCullen, I.D. Johnson and E.W. Sheppard, Chem. Mater., 6 (1994) 2070.
(1992) 710.
3. 4.
100
10. 11. 12. 13. 14. 15. 16. 17. 18 19.
20. 21. 22. 23.
J.C. Vartuli, K.D. Schmitt, C.T. Kresge, W.J. Roth, M.E. Leonowicz, S.B. McCullen, S.D. Hellring, J.S. Beck, J.L. Schlenker, D.H. Olson and E.W. Sheppard, Chem. Mater., 6 (1994) 2317. P.J. Branton, P.G. Hall and K.S.W. Sing, J. Chem. Soc., Chem. Commun., (1993) 1257. A. Corma, V. Fornes, H. Garcia, M.A. Miranda and M.J. Sabater, J. Am. Chem. Soc., 116 (1994) 569. A. Corma, M.T. Navarro and J.P. Pariente, J. Chem. Soc., Chem. Commun., (1994) 147. K.M. Reddy, I. Moudrakovski and A. Sayari, J. Chem. Soc., Chem. Commun., (1994) 1059. P.T. Tanev, M. Chibwe and T.I. Pinnavaia, Nature, 368 (1994) 321. T. Blasco, M.T. Navarro and J.P. Pariente, J. Catal., 156 (1995) 65. S. Gontier and A. Tuel, Zeolites, 15 (1995) 601. A. Sayari, C. Danumah and I.L. Moudrakovski, Chem. Mater.,7 (1995) 813. Z.Y. Yuan, S.Q. Liu, T.H. Chen, J.Z. Wang and H.X. Li, J. Chem. Soc., Chem. Commun., (1995) 973. D. Zhao, and D. Goldfarb, J. Chem. Soc., Chem. Commun., (1995) 875. P.K. Vinson, J.R. Bellare, H.T. Davis, W.G. Miller and L.E. Scriven, J. Colloid Interface Sci., 142 (1991) 74. C.Y. Chen, S.L. Burkett, H.S. Li and M.E. Davis, Microporous Mater., 2 (1993) 27. R. Schmidt, M. Stocker, D. Akporiaye, E.H. Torstad and A. Olsen, Microporous Mater., 5(1995) 1. A. Zecchina, G. Spoto, S. Bordiga, A. Ferrero, G. Petrini, G. Leofanti and M. Padovan, Zeolite Chemistry and Catalysis, ed. P. A. Jacobs, N.I. Jaeger, L. Kubelkova and B. Wichterlova, Elsevier, Amsterdam, 1990, p. 251. Y.L. Kim, R.L. Riley, M.J. Huq, S. Salim, A.E. Le and T.E. Mallouk, Mat. Res. Soc. Symp. Proc. 233 (1991) 145. A. Thangaraj, R. Kumar, S.P. Mirajkar and P. Ratnasamy, .1. Catal., 130 (1991) 1. R.A. Sheldon, J. Mol. Cat., 7 (1980) 107. R. Kumar, G.C.G. Pais, B. Pandey and P. Kumar, J. Chem. Soc., Chem. Commun., (1995) 1315.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105 1997 Elsevier Science B.V.
101
S H O R T R A N G E ORDER OF MCM-41 A N D M E S O S T R U C T U R E D ALUMINIUMPHOSPHATE
C. Pophal, R. Schnell, H. Fuess FB Materialwissenschaft, Fachgebiet Strukturforschung, TH Darmstadt, Petersenstr. 20, D-64287 Darmstadt, Germany
The X-ray amorphous walls of MCM-41 possess a well defined short, but also a middle range order. The addition of Ti or AI to the synthesis gel of MCM-41 does not significiantly affect the short and middle range order of the walls. Mesolamellar aluminiumphosphates can be prepared by the liquid crystal templating (LCT) method. The aluminium atoms are within a tetrahedral coordination of oxygen.
Keywords Mesoporous, MCM-41, aluminiumphosphate, WAXS.
I. Introduction Since their discovery by the Mobil Oil Corporation 111, mesoporous inorganic materials, especially MCM-41, are extensively studied. Several mesostructured inorganic compounds, e. g. transition-metal oxides have been prepared and characterized 12-31. In the course of our investigations we have synthesized mesostructured aluminiumphosphate using the LCT mechanism. The sample has been analysed by X-ray powder diffraction (XRD), transmission electron microscopy (TEM) and thermal analysis (TGA). To elucidate the structural organisation of the inorganic walls, we have investigated calcined purely silica MCM-41, AI-MCM-41, TiMCM-41 and as-prepared mesostructured aluminiumphosphate by wide angle X-ray scattering (WAXS). This method provides a radial distribution function (RDF) from the corrected experimental X-ray data without any a priori assumptions of the atomic arrangement. Interatomic distances and angles are directly derived from the RDF. Additional 27A1- and 3 Ip_ MAS NMR measurements were performed to check and complete the results obtained by WAXS on aluminiumphosphates.
102
2. Synthesis 2.1. MCM-41 Samples containing AI were prepared as described by Chen et al. [4]. The Si/AI molar ratios in the reaction mixtures were fixed to oo, 30, 28 and 17, respectively. Ti-MCM-41 with a Si/Ti ratio of 52 was synthesized following the procedure reported by Corma et al. [5]. All MCM-41 molecular sieves were prepared using hexadecyltrimethylammoniumchloride (25%, Fluka) as template. The as-prepared samples were washed with water and calcined for 12 hours at 540~ to remove the organic surfactant.
2.2. Aluminiumphosphate An aqueous solution of pseudoboehmite (aluminiumoxide-hydrate containing 74% A1203, Condea) and ortho-phosphoric acid (85%, Merck) was combined with an aqueous solution of hexadecyltrimethylammoniumhydroxide (Fluka). The mixture was stirred at room temperature and placed in a static autoclave at a temperature of 150~
for two days. The product was
recovered by filtration on a Buchner funnel, washed with water, and dried in air at ambient temperature. The pH-value was adjusted by addition of the template. Best results were obtained in the pH range between 8 and 11 161.
3. Analysis The XRD data at room temperature were collected on a powder diffractometer described by Hsu et al. 171 using CUKal radiation. Data were taken in the angular range of 1~ to 11 ~ (20). The transmission electron micrographs were performed on a Philips CM-20 transmission electron microscope operated at 200kV. To increase the contrast the picture of MCM-41 was taken at strong underfocus. Thermogravimetric analyses were carded out on a TGA 92-18 in the temperature range from 293K up to 1673K. The data for the WAXS investigations were taken from 3 ~ to 140~ (20) using MOKal radiation. For the data collection a scintillation counter was used with an integration time of 400s per data point in steps of 0.05 ~ The influence of the special sample environment (quartz-glass capillary, diameter 0.5mm) has been determined by measuring the background scattering caused by the empty capillary. The observed intensities were corrected, both for absorption and polarization according to Paalman and Pings [81, using the LASIP software package from Lecante 19]. The corrected intensities were normalized by the method of Kroegh-Moe [10]. Finally, the RDF has been obtained by Fourier transformation of the corrected and normalized intensifies. The MAS NMR spectra were recorded at room temperature on a Bruker MSL-400 spectrometer.
103
4. Results and discussion 4.1. MCM-41
The obtained XRD patterns from the as-prepared and calcined samples are in excellent agreement with the data reported by Beck et al. 111. Direct TEM imaging unambigously reveals the regular array of uniform channels, which are the main characteristic of MCM-41. A representative TEM image is shown in Figure 1. The d~00-spacing for all as-synthesized samples is about 40A. The high temperature treatment of the samples during the calcination reduces the mean pore diameter by about 10%, as described by Janicke et al. [11]. As a paradigm case, the radial distribution function of as-synthesized, purely siliceous MCM-41 obtained by WAXS is shown in Figure 2 and will be discussed. The RDF reveals spurious maxima corresponding to distances smaller than 1A due to series termination effects. The first concentration of electron density is assigned to the average Si-O distance and appears at 1.60A. Distances of two oxygen atoms within a SiO4-tetrahedron are observed at 2.60A. The average electron density of two silicon atoms of comer-sharing SiO4-tetrahedra appears at 3.05A. This implies, under the assumption of regular tetrahedra, an average Si-O-Si angle of 145 ~ Based on crystal chemical considerations, the distances in the RDF up to 3A can easily be assigned. Most remarkable are the rather sharp peaks in the RDF. This clearly reflects a high degree of short and middle range order within the inorganic walls.
~ '~'~' ~ ~ " .~ ,~ ~'~, .~ ~9
~_~
j
~..
9' ~ , i i ~ i
~
i~. "....~";.~,~;. '.i~ .~,,% ".,-, "~' " " ' ~.,~:.-.,~.r ....., ~ ..... ~.~'~' ".,~
~"
~
~"
"
looA Figure 1. Transmission electron micrograph of calcined purely siliceous MCM-41.
104
11~ ,,-..,.,,
=
5000
a
-5000
' ' '
2
0
4
6
a [,N
8
10
Figure 2. RDF of calcined purely siliceous MCM-41. Interatomic distances caused by the surfactant do not contribute significantly to the RDF, due to its rather low scattering strength and concentration. The RDF of the samples with incorporated A! and Ti do not reveal significant differences compared to purely siliceous MCM-41.
4.2. Aluminiumphosphate The XRD pattern recorded, reveals three reflections in the angular range 1~ to 11~ (20), which correspond to a lamellar phase with do01 of 31A (Figure 3). The periodic lamellar arrangement of the inorganic layers is also confirmed by direct TEM imaging. The TGA analysis indicate a ratio of suffactant to Al of about 3.5.
'
I
'
'
400
'
001
I
'
'
'
I
'
'
'
I
'
'
"
I
'
300 .n t/) r-
Q) t---
n
200 100 I L l ,
, 2
002 ~ .
L_ _ ~ l
.
4
.
.
.
6 20
_ 003 L....r-.
8
'
.--!--
'--
10
Figure 3. XRD pattern of as-prepared lameUar aluminiumphosphate with a mean d-spacing of 31A.
105
. .
,~,
.,
...
~.,,..
,.,
9
..
~
. ?
..
... . . . .
...'
,.
Figure 4. Transmission electron micrograph of as-prepared lameUar aluminiumphosphate. The radial distribution function obtained by WAXS is displayed in Figure 5. Model calculations, based on the data of berlinite, were performed in order to assign the observed intensities in the experimental RDF to interatomic distances.
110 4
"E
5000
*"
0
.IQ L_
'
9
9
II
|
II
g
II
|
g
,
,
,
9
9
9
U.
a
n-
-5000
-1 10 4
9
,
9
I
2
,
9
9
I
4
R
[A]
I
,
,
6
Figure 5. RDF of as-prepared lamellar aluminiumphosphate.
.
I
8
,
'
I
10
106 The RDF reveals rather sharp electron concentrations. This indicates a narrow distribution of interatomic distances and a high degree of short and middle range order. The electron density at 1.60A is assigned to the average distance of aluminium and phosphorous to oxygen atoms within a tetrahedral arrangement. Because of restrictions caused by the experimental resolution, it is not possible to distinguish between AI-O and P-O distances. AI is tetrahedrally coordinated, since no electron density around 1.80-2.00A is observed. The maximum at about 2.55A is attributed to the average distances of two oxygen atoms within PO4- and AIO4-tetrahedra. This implies, under the assumption of regular tetrahedra, an average AI-O-P angle of 145~
l .
.
.
.
!
80
1
. . . .
60
:
l I
9 J
40
J
J
,
J
PPM
20
J
]
J
I
0
J
J
....
1
-20 '-
,
,
J_
-40
:
-
Figure 6. 27AI-MAS NMR spectrum of as-prepared lamellar aluminiumphosphate.
1
_
I
0
.L
I
-5
.
I
-I0
l,
I
-15
I
-20
1
PPM
-25
t
-30
I
-35
.l
I
-40
!
-45
,
Figure 7.3 IP_MA S NMR spectrum of as-prepared lamellar aluminiumphosphate.
I
i
107 Within this structural model all distances up to 5A as derived from the experimental RDF can be explained. The observed maxima at distances above 5A cannot be uniquely assigned to interatomic distances, because of the increasing number of contributions to the electron density. The 27Al-MAS NMR spectrum (Figure 6) consists of one broad signal with a chemical shift of 40ppm, which corresponds to the 27A1 chemical shifts for solid A1PO4 compounds in which Al is covalently bound to four P atoms via oxygen bridges [12]. This implies the absence of octahedrally coordinated Al. The peak is asymmetric, due to AIO4-tetrahedra which are linked to less than four PO4-tetrahedra. The broadening of the signal implies a certain distribution of angles within the tetrahedral coordination around Al. Therefore, the calculated AI-O-P angle derived from the RDF can only be seen as an average angle. The lack of strong sidebands and the sharp maxima in the RDF indicate a high degree of short range order. The 31P_MAS NMR spectrum (Figure 7) shows three strong peaks at -17ppm, -21ppm and -29ppm. In the range of -25 to -30ppm most of the signals of phosphorous atoms with four covalent oxygen bridges to aluminium are observed in the various crystalline forms of aluminiumphosphate 1111. The signals at -17ppm and -21ppm are caused by phosphorous atoms with mixed coordination P(OH)x(OAI)4_x.
5. Conclusion Our WAXS investigations reveal a high degree of short and middle range order of the inorganic walls of silica-MCM-41, AI-MCM-41, Ti-MCM-41 and lamellar aluminiumphosphate. The addition of AI or Ti (ratio see 2.1.) to the synthesis gel does not significantly affect the structural organisation of the walls of MCM-41. With regard to the coordination of AI within the aluminiumphosphate layers, solid-state NMR studies support the result obtained by WAXS. Modified Rietveld refinements, using the program ARITVE from Le Bail [13] are in progress to obtain an improved model for the structural organisation of the inorganic walls of MCM-41. This method is a variation of the reversed Monte Carlo technique (RMC). It has been successfully applied to the least squares refinement of glassy SiO2. In-situ experiments are in progress and expected to provide the
experimental
background for an improved
"understanding" of the structural alterations during the formation of MCM-41 and other mesostructured inorganic materials.
Acknowledgment We thank Dr. Engelhardt and M. Feuerstein at the Universit~t Stuttgart for the performance of the 27A1- and 31p_MAS NMR measurements, Dr. Stamm at the Max Planck Institut Mainz for providing of XRD equipment and Dr. Franke and Prof. Schulz-Eckloff at the Universit~t Bremen for the support on aluminiumphosphate.
108 References
C. T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli, J. S. Beck. Nature, 359 (1992) 710. .
U. Ciesla, D. Dehmut, R. Leon, P. Petroff, G. Stucky, K. Unger, F. Schiith. J. Chem. Soc., Chem. Commun., (1994), 1387.
.
Q. Huo, D. I. Margolese, U. Ciesla, P. Feng, T. E. Gier, P. Sieger, R. Leon, P. M. Petroff, F. SchUth, G. D. Stucky. Nature, 368 (1994) 317.
.
5.
C.-Y. Chen, H.-X. Li, M. E. Davis. Microporous Mater., 2 (1993) 17. A. Corma, M. T. Navarro, J. P6rez-Pafiente, F. Sanchez. Studies in Surface Science and Catalysis, Vol. 84 (1994) 69.
.
7.
R. Schnell. Diplomarbeit, TH Darmstadt (1994). T. C. Hsu, B. Hiiser, T. Pakula, H. W. Spiess, M. Stamm. Makromol. Chem., 191 (1990) 1597.
~
H. H. Paalman, C. J. J. Pings. Appl. Phys., 33 (1962) 2635.
9.
P. Lecante. Th~se at the Centre National de la Recherche Scientifique Toulouse, (1990).
10.
J. Kroegh-Moe, Acta Cryst., 9 (1956) 951.
11.
M. Janicke, D. Kumar, G. D. Stucky, B. F. Chmelka. Studies in Surface Science and Catalysis, Vol. 84 (1994) 243.
12.
M. A. Harmer, A. J. Vega. Solid State Nuclear Magnetic Resonance 5 (1995) 35.
13.
A. Le Bail. Journal of Non-Crystalline Solids 183 (1995) 39.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
109
Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
Syntheses of mesoporous aluminosilicates from layered silicates containing aluminum. S. Inagaki, Y. Yamada and Y. Fukushima Toyota Central R&D Labs., Inc., 41-1, Nagakute, Aichi, 480-11, JAPAN Addition of Al(NO3)3~
or NaAIO 2 as an AI source formed crystalline layered sodium
silicates containing AI. Aluminosilicate mesoporous molecular sieves were synthesized by heating
the
layered
sodium
silicates
with
various
amounts
of
AI
in
hexadecyltrimethylammonium chloride solution. The mesoporous aluminosilicates with hexagonal regularity and uniform pore-size distribution had only tetrahedral Al in the framework and large amount of acidity. Although the addition of Al(NO3)3~
formed not only the
layered sodium silicates but also cristobalite (SiO2) crystal, the addition of NaA10 2 formed no crystobalite. It suggested isomorphous substitution of Al for Si in the SiO 2 framework of the layered sodium silicates and the mesoporous materials. 1. INTRODUCTION Mesoporous molecular sieves such as MCM-411) and FSM-162) have attracted much attention, because of their applicability to catalysts and adsorbents for large size molecules. FSM-16 is synthesized from a layered sodium silicate by using surfactants 3). A folded sheet mechanism has been proposed for the formation of FSM-16 3'4).The topochemical synthetic method of FSM16 is expected for a new strategy for synthesizing various inorganic materials. Several attempts 5-9)have been made to incorporate AI in siliceous framework of the mesoporous materials and apply the aluminosilicate mesoporous materials to various catalytic reactions such as a synthesis of porphyrin 1~ Although aluminosilicate MCM-41 materials containing only tetrahedral Al in the framework have been synthesized, their structural regularity were lower than those of silicious MCM-41 materials 6'7). Only one or two peaks at a low angle region in X-ray diffraction patterns were observed for the aluminosilicate MCM-41 materials with a relatively low Si/Al ratio under 50. The structural regularity decreased with increasing Al contents and their diffraction peaks due to the hexagonal regularity disappeared for the samples with the Si/
110 AI ratios of 26) or 57). We also reported that an impregnation of FSM-16 with aluminum chloride aqueous solution produced a mesoporous aluminosilicate 5), although, the mesoporous materials contained AI in not only a tetrahedral site but also an octahedral site. The amount of acid was about an half of that on ZSM-5 with the same AI203 contents. Here we have tried to synthesize aluminosilicate mesoporous molecular sieves with high regularity and only tetrahedral AI from a layered sodium silicates containing AI. 2. EXPERIMENTAL
2.1. Preparation of Layered Sodium Silicates Containing Aluminum. Aqueous solutions of Al(NO3)309H20 or NaAIO 2 were added in sodium silicate aqueous solution (SiO2/Na20=2), and the mixtures were stirred at 50* C for 3h. The solutions were dried at 100 *C for 12h and vacuum-dried at 70 *C for 12h to yield sodium aluminosilicate glasses. The glasses were calcined at 700 *C for 6h to crystallize to layered sodium silicates containing AI. The Si/AI molar ratio in the initial mixtures ranged from 2.5 to 100 as listed in Table 1.
2.2. Conversion to Mesoporous Aluminosilicates. The layered sodium silicates were dispersed in water and stirred at room temperature for 3h. The filtered samples (50 g) were dispersed in 0.1 mol dm3 hexadecyltrimethylammonium chloride aqueous solution (1000 cm 3) and heated at 70 *C for 3h. 2N HC1 aqueous solution was added to the dispersion to adjust the pH value to 8.5, and they were maintained at 70 ~ for further 3 h. The filtered samples were dried at 60 ~ and calcined at 550 ~ for 6 h to remove organic fractions. Consequently, we got Al-containing FSM-16 samples with the bulk Si/AI molar ratio between 7.2 and 188 as listed in Table 1. The Si/AI ratios in the Al-containing FSM-16 materials were determined by inductively coupled plasma-atomic emission spectrometry. The higher Si/A1 ratios of the final products than the initial solutions were due to a dissolution of A1 during the dispersion of the layered sodium silicates in water.
2.3. Characterizations. X-ray powder diffraction pattems were obtained
by
using
a
Rigaku
RAD-B
Table 1 AI sources and Si/A1 molar ratios. Si/A1 ratio A1 sources
Initial solution 100 AI(NO3)3"9H20 50 20 5 4 NaAIO2
50 5 2.5
Final products 188 67 38 9.9 7.7 132 12 7.2
111 diffractometer with Cu-Kct radiation 9 Solid state MAS NMR spectra were measured on a Bruker MSL-300WB spectrometer 9 295i MAS NMR spectra were recorded at a frequency of 59.620 MHz spinning 4 kHz using pulses at 90-s intervals and 360 scans 9 27A1MAS NMR spectra were recorded at a frequency of 78.205 MHz spinning 4 kHz using pulses at 2-s intervals and 1000 scans. Ammonia-TPD spectra were measured with a conventional TPD apparatus, in which the desorbed materials were detected by a thermal conductivity detector. About 0.1 g of the samples were vacuum-dried at 500* C for lh. The dried samples were then exposed to 13.3 kPa of an ammonia gas at 100 ~C for 45 min, followed by evacuating at 100 ~C for lh. The TPD spectra were measured from 100 ~ to 1000 *C at a heating rate of 10 ~C/min. in a helium flow as carrier gas controlled at 4.0x10 3 of W/F.
3. RESULTS AND DISCUSSION Figs. 1 and 2 show X-ray diffraction pattems of Al-containing FSM-16 prepared by using Al(NO3)3 9
and NaAIO z as AI sources 9 The FSM-16 samples with Si/A1 ratios of 188, 132,
9cristobalite
/ 8 r
1..8i~ ' /] -t / :
~
~,,~,~,,.~_~__'
10 20 20 (CuKa)
30
67 / .."
/
-
/ /
38 ~
....9..,.9.....
....7..,2... 10
40
Figure 1. X-ray diffraction patters of aluminosilicate FSM-16 materials various Si/A1 ratios prepared by using AI(NO3)a.9H20 as AI source.
112
,
0
5
10
.
.
10
1
3
2
"
20
' ~
30
40
20 (CuKet) Figure 2. X-ray diffraction patters of aluminosilicate FSM-16 materials various Si/AI ratios prepared by using NaAIO 2 as A1 source.
67, 38 and 12 showed three Or four obvious peaks assignable to hexagonal symmetry at an angle smaller than 10 ~ The diffraction patterns indicate that their structural regularities were higher than those of MCM-41 materials with the same Si/AI ratio reported previously6-9). For the samples with the Si/A1 ratio of 9.9, though the peak intensity was reduced, two or three peaks were still observed in a low angle region, which suggested preservation of hexagonal regularity. The unit cell dimensions of the samples prepared by using AI(NO3)3-9H20 decreased from 4.3 to 4.0 nm with decreasing the Si/A1 ratio from 188 to 9.9. Those of the samples with the Si/A1 ratios of 132 and 12 prepared from NaAIO 2as an AI source were 4.4 nm. While, the products with the low Si/AI ratios of 7.7 and 7.2 showed only one broad peak in a low angle region. On the othe hand, the product (Si/AI=7.7) prepared from AI(NO3)3-9H20 showed several peaks due to the other crystal in a high angle region. Those peaks were assigned to sodium aluminum silicate hydroxide hydrate crystal. FSM-16 materials were not formed in such a high AI content, which was attributable to using non-layered sodium silicates as starting materials formed from the sodium aluminosilicate glasses mentioned later. Diffraction peaks due to cristobalite crystal were also observed in a higher angle region for all the samples prepared by using AI(NO3)3"9H20, and their intensity was increased with increasing the added amount of AI(NO3)3.9H20. The samples prepared by using NaA102 had almost no formation of cristobalite as shown in Figure 2. These results suggested that the introduction of A1 ions into
113 the sodium silicates without any supply of Na ions expelled Si from the framework of the layered sodium silicate and FSM-16.
The AI introduction incorporating with Na formed sheet
silicates including A1 and FSM-16 without ejecting Si to form crystobalite crystals, which is represented by the following chemical equations, (1) and (2). Na2Si205 + xAI(NO3)3 + (3x/2)H20 ---> Na2Si2.xAl H30s +xSiO 2 +3xNO 2 +302
(1)
(1-x)Na2Si20 s + (2x)Na~O 2 + xH20 -> Na2Si2zAl2xH2xOs
(2)
4-AI
03 04 9
i
/AI= 12
/A,J= 38 ,
,
200 100
0 -100 -200 ppm Si / AI m
-
m
-
u
-
-80
|
-
u
-
-100 ppm
u
-120
Figure 3. ZrAl and 29Si MAS NMR spectra of as-synthesized FSM-16 materials. The FSM-16 samples with Si/AI ratios of 12 and 38 were prepared by using NaAIO 2 and AI2(NO3)a'9H20, respectively. At
o' /Al = 12 I
~
i
/
A
l
= 38
200 100 0 -100-200 ppm Si / Al 9
.
,
-80
.
,
-
,
-
-100 ppm
,
.
9
-120
Figure 4. 27A1and 29Si MAS NMR spectra of calcined FSM-16 materials. The FSM-16 samples with Si/AI ratios of 12 and 38 were prepared by using NaAIO 2 and AI2(NO3)3~ O, respectively.
114
6- Na2Si20 5
Cristobalite---
~
~
~ . . . .
_
=
1
8
8
=
.
9.9 . . . .
10
;0 20(CuKet)
Figure 5. X-ray diffraction patterns of calcined products at 700 ~C of aluminosilicate glasses with various Si/AI ratios prepared by using A12(NOa)a~
These results strongly suggest that AI is incorporated in the silicate framework of the layered sodium silicates and the FSM-16 materials. BET surface areas were 800-1300 mZ/g for the Al-containing FSM-16 samples and 30-300 m2/g for the sodium aluminum silicate hydroxide hydrate crystals. NMR spectra of the as-synthesized FSM-16 samples and the calcined samples are shown in Figures 3 and 4. 27A1MAS NMR spectra of the Al-containing FSM-16 samples with the Si/A1 ratios of 38 and 12, prepared by using Al(NOa)3*9H20 and NaAIO2 as A1 sources respectively, showed almost only one signal due to tetrahedral AI before and after calcination. Broadening of the signal during calcination suggesting somewhat dealumination from the framework was obObvious broadening was not observed served for the sample prepared by using AI(NO 3)3~ for the sample prepared by using NaA102, which suggested its higher thermal stability than the sample prepared by using Al(NOa)a~ The incorporation of A1 in the silicious framework was also confirmed by 29SiMAS NMR spectra. Lower shifts at 3-7 ppm of signals assigned to Q3 and Q4environmental SiO4were observed for both as-synthesized and calcined samples after introduction of AI as shown in Figures 3 and 4. Such a peak shift was also observed for zeolites with Si (OSi)3(OA1). Figure 5 shows X-ray diffraction patterns of the calcined sodium aluminosilicate glasses prepared by using AI(NO3)3~
The diffraction patterns due to a layered sodium silicates, 6-
Na2Si205 were observed for the calcined products with Si/AI ratio over 9.9, while those were
115
|
[-
l~ "6~
|
IF
l
ii
(This work)
//
== 0.5~[ /
'
FSM-16
)llrSi/Al=9.9
0""""
FSM-16
I
(Impregnation)
o ........
..O ......
silica-alumina
<
0.0 0
10
20
30
AI20 3 contents (wt%) Figure 6. Relationship between amount of acid and AI203 contents of various aluminosilicate materials determined by NHa-TPD. hardly observed for the samples with the low Si/AI ratio of 7.7. Cristobalite was contained in the layered sodium silicates, and its content increased with added amount of AI(NOa)a.9H20 as shown in Figure 5. Although 6-Na2Si205 crystal also formed in the calcined products prepared by using NaAIO 2with the Si/Al ratio higher than 12, cristobalite did not formed in all samples. These results support the expelling of Si from the framework of the layered sodium silicates mentioned above. The d-spacings of the diffraction peaks of those layered silicates containing Al were similar to those of •-Na2Si205. Acid amounts of the aluminosilicate FSM-16 materials were larger than those prepared by impregnating aluminum chloride solution and usual amorphous aluminosilicate with the same Si/Al ratio reported previously~3as shown in Figure 6. The acid amounts were 0.7 times of those of ZSM-5. It indicates highly level incorporation of Al in the framework of FSM-16 prepared from the layered silicate containing Al. NHa-TPD profiles of the aluminosilicate FSM-16 materials resembled in those observed in amorphous aluminosilicates, which suggested broad distribution of acid-strength. The successive formation of mesoporous molecular sieves with high regularity and high alumina would be attributable to using a layered silicate containing Al as starting material, although further studies are necessary to clarify the mechanism.
116 4. CONCLUSION The aluminosilicate mesoporous molecular sieves with high alumina and highly regular structure were prepared from layered sodium silicates containing A1. The expelling of Si from the framework of the layered silicates, the large amount of acidity and the NMR results indicated the high level incorporation of AI in the framework of the FSM-16 materials. REFERENCES
1) C. T. Kresge, M. E. Leonowicz, W. J. Roth, J. C. Vartuli, J. S. Beck,, Nature, 359 (1992) 710. 2) S. Inagaki, Y. Fukushima, K. Kuroda, J. Chem. Soc., Chem. Commun., (1993) 680. 3) S.Inagaki, A. Koiwai, N. Suzuki, Y. Fukushima, K. Kuroda, Bull. Chem. Soc. Jpn, in press. 4) S. Inagaki, Y. Fukushima, K. Kuroda, In Zeolite and Related Microporous Materials: State of the Art 1994, Eds. J. Weitkamp, H. G. Karge, H. Pfeifer, W. Holderich, Elsevier, (1994) 125. 5) S. Inagaki, Y. Fukushima, A. Okada, T. Kurauchi, K. Kuroda, C. Kato, Proceedings from the Ninth International Zeolite Conference, Montreal 1992, I, 305. 6) R. B. Borade, A. Clearfield, Catal. Lett., 31 (1995) 267. 7) Z. Luan, C-F. Cheng, W. Zhou, J. Klinowski, J. Phys. Chem., 99 (1995) 1018. 8) A. Corma, V. Fornes, M. T. Navarro, J. Perez-Pariente, J. Catal., 148 (1994) 569. 9) K. R. Kloetstra, H. W. Zandbergen, H. van Bekkum, Catal. Lett., 33 (1995) 157. 10) T. Shinoda, Y. lzumi, M. Onaka, J. Chem Soc., Chem. Commun., (1995) 1801.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved 9
117
STRUCTURE DESCRIPTORS FOR ORGANIC TEMPLATES EMPLOYED IN Z E O L I T E S Y N T H E S I S R E Boyett,* a,b A P Stevens, a,b M G Ford b and P A Cox a,b Division of Chemistry, University of Portsmouth, St. Michaels Building, White Swan Road, Portsmouth, Hants, PO 1 2DT, UK. b Centre for Molecular Design, University of Portsmouth, Halpem House, 1/2 Hampshire Terrace, Portsmouth, Hants, PO 1 2QF, UK. a
ABSTRACT
A structural analysis has been carried out upon 130 organic templating agents employed in the synthesis of zeolites from 18 different framework types. The orthogonal principal axes of inertia of these molecules provide quantitative structure descriptors which can be plotted to produce three-dimensional 'shape-space' diagrams. Groups of templates which produce different zeolite framework architectures plot in discrete areas of these graphs. If the set of templates for a single framework type occupy more than one region of this shape-space, it can indicate that several modes of incorporation are found for the template molecules within the relevant zeolite porespace. Large, complex templates can often be demonstrated to comprise multiple structural units, or sub-shapes, the latter having similar dimensions to the smallest agents in any one set of templates, i.e. those that fulfil the minimum void-filling requirements of particular pores. Regions of overlap may occur between whole families of templates in the principal axes of inertia shape-space. The templates which plot within an overlap region may direct the formation of any of the different zeolite frameworks whose template shape-space envelopes interpenetrate at that point. The actual outcome of syntheses that deploy templates from these regions thereby depend more critically than usual upon factors besides just template shape, such as the composition of the reaction media and the reaction conditions. The quantitative description of template size and shape afforded by the use of principal axes of inertia highlights the importance of template shape in determining the zeolite product formed.
1. INTRODUCTION
Zeolite catalysts are being synthesised to an increasing extent via the use of gels that contain specific organic templating or structure directing agents. The exact r61e which these agents play in zeolite formation has not been established, but previous research has shown the size and the shape of any particular template molecule to be an important factor in defining the lattice structure of the eventual zeolite product, t1'2'3'4]as, indeed, is the template orientation. [51 9
118 Although a number of molecular modelling techniques have been applied in zeolite research, [6'7~none have yet provided a tool facilitating the quantitative description of template structure. In order to address this need we have investigated techniques that have a proven record in the disciplines of Quantitative Structure-Activity Relationships (QSAR), I8~ and drug design, applying the lock and key analog)Jg~ for the conformational interaction between drug and receptor site in a novel way, to rationalise the relationship between the structures of template molecules which direct the formation of the same products. Several different properties are suitable for the task of structure representation, t1~ the present study has employed the molecular principal axes of inertia. The results discussed below identify such descriptors as potential aids to our understanding of template-framework relationships, and we discuss their potential for application in the rational design of novel materials.
2. E X P E R I M E N T A L
Structure analysis was carried out upon 130 organic templating agents which have been employed in 229 syntheses documented in research literature and in patent applications. [1il The zeolites formed using these 130 agents exhibit 18 different framework structures; all examples investigated here were of a siliceous or aluminosilicate composition, and our conclusions are therefore restricted to zeolite-template systems of this type. Molecular mechanics calculations were used to defme a low potential energy conformation for each molecule, utilising the potentials and parameters in the CVFF force field, implemented within the program Discover. c12! The orthogonal principal axes of inertia, RN, were calculated using the Tsar Quantitative Structure-Activity Relationships (QSAR) software, t13~ These quantities are customarily described in ,~mgstroms, and define an ellipsoid (see Figure 1) which is scaled in inverse proportion to the molecular moments of inertia for a given template. RY
cr---
~
i
~
- - ~ '
RX
Figure 1. Inertial ellipsoid for a typical template molecule. The dimensions of the ellipsoid, RN, are inversely proportional to the molecular moments of inertia, IN. Two assumptions have been made in order to apply the principal axes of inertia in this way. Firstly, the derived molecular conformations are taken to represent those of templates located inside pore systems, without the explicit consideration of either thermal motion or of any conformational change of the template within the host arising from lattice-template interaction. Secondly, the masses of the C, N, and O atoms defining the 'backbones' of the templates are considered to be similar enough to permit a direct comparison of moments, and therefore RN values, between all molecules in the survey. These assumptions do not affect the employment of principal axes of inertia as a tool to describe the structure of templates at a first
119 approximation, indeed, the axes retain inherent advantages over alternative shape descriptors, being convenient to calculate, and requiring no pre-alignment, or definition of reference atoms.
3. RESULTS AND DISCUSSION The use of a template during zeolite synthesis can impart a very strong influence on the pore architecture developed within an eventual product. The extent to which the influence is controlled by the shape of the template is illustrated in the three-dimensional plots below, which depict the principal axes of inertia for several systems. The templates making different products are found to occupy discrete RN 'shape-space.' It should be noted that a little distinction is lost owing to the reduction of the 3-D plot onto a plane projection, and that only a limited groups of structures may be included in any one plot without significant loss of clarity. The data shown in Figure 2 represent six different framework types in which the templates are enclosed in clearly defined shape-space, this degree of enclosure may be rationalised quite simply. For example, the templates that form the cage-like cavities in NON-type zeolites are small molecules whose structures essentially occupy a spherical or toroid volume, agents such as adamantanes and unsaturated ring compounds, respectively. These molecules share similar RN values, where all three components are of approximately the same magnitude. The other framework types depicted in the figure are also shape specific in their templating requirements. Docking studies t4] indicate that only molecules of very precise dimensions may locate within the pockets along the pores of zeolite EU-1 (EUO). Similarly, the templates found to direct the crystallisation of zeolites ZSM-18 (MEI) and ZSM-57 (MFS) are seemingly very few, and occupy small, specific volumes of shape-space on the graphs. This is arguably because only very few compounds have the correct size and shape to direct the formation of these particular pore architectures. 4 3.6 3.2 2.8
i
11a
I !
I
2.4
m
ml
m
m
I
ml
m
1.2
0
2 RY
4
6 ~
lo lOO
80
60
40
20 RX
Figure 2. Principle axes of inertia (]k) for templates that produce zeolites assigned to the framework categories" NON ~ , MEL IlL EUO O, LEV &, MEI 1r and MFS ~.
120
All but one of the agents represented in Figure 2 and which form the MEL-type structure are homologous linear diamines which exhibit closely related RY and RZ values but have large and variable RX components, such that they plot as a parallel band in the figure. These templates are encapsulated along straight pore channels in ZSM-11 and its analogues. In contrast, tetrabutylammonium, whose RX and RY values are identical but whose RY and RZ values are comparatively larger than the diamines, is located centrally at pore intersection sites. The principal axes of inertia can clearly distinguish between these different modes of template accomodation within one pore system, as well as between framework varieties, evidence for such modes arising from the division of the shape-space for a given template set into subregions, one being found for each mode.
2.4 2.2 2
1.8 1.6 1.4 1.:
I
100
80
ou
--
RX
Figure 3. Principle axes of inertia (/~) of templates making up zeolites with MTT frameworks. Templates are coded thus: ,ik basic unit, occupying a single lobe; Ill double unit, occupying two lobes; and 9 multiple lobe-occupying units. Table 1. Maximum and minimum values for principal axes of inertia of templates which form zeolites with a MTT type framework.
Lobes occupied
Value
R X / / ~ RY / A R Z / A
Surface Molecular Area/]k z V o l u m e / A 3
Single
Max Min Only Max Min
11.9 2.7 25.8 97.0 39.0
108 82 167 378 290
Double Multiple
2.70 1.47 1.50 2.24 2.21
1.56 1.31 1.46 2.23 2.21
63 44 97 269 203
Unidimensional zeolite pore systems may exhibit several modes: there are at least three ways in which templates can be incorporated within the pores of zeolites which have the MTT-
121 type pore system, (e.g. ZSM-23). In addition, this framework type can also be used to introduce the concept of template shape and 'sub-shape.' The five smallest templates represented in Figure 3 and Table 1 can effectively be considered as void-filling traits ('mode 1') whose shape and molecular volume, c. 50 A, define the most basic requirements for the unidimensional MTT pore channels, with their regularly spaced, undulating lobes. Figure 4 illustrates the relationship of two small templates to these pore lobes, the organic agents pyrrolidine and 2-aminoethanol having been docked into the channels manually using computer graphics. The poremap in this and other similar figures has been defined by showing the space accessible to a template after van der Waals surfaces have been generated around the zeolite's framework. The other templates in the MTT set occupy more than one pore lobe, either by spanning two adjacent lobes (dipropylamine, 'mode 2') or by bridging between more distant cavities (as do the diammonium ions, 'mode 3'). The basic units such as pyrrolidine may therefore be envisaged as effective sub-shapes of the larger compounds. The four diammonium compounds typify a feature frequently seen amongst sets of templates in our investigation, in that they comprise a co/nmon chemical form with repeated structural units, and their total volume is approximately a multiple of that found for the basic void-filling templates, (Table 1). Only heptamethonium is shown within the pore in the figure, although presumably the other agents, octa-, undeca- and dodecamethonium, are accomodated in a closely-related fashion, with their quarternary nitrogen centres housed in pore lobes. It is not clear from Figure 4 whether nona- and decamethonium are unable to produce MTT systems in this way, or whether they have .been used successfully to synthesise such structures but were simply not identified in our primary search of the literature. If the lobe spacing does restrict the alkyl chains linking the nitrogens in diammoniums to certain permitted lengths, it appears from the figure and table that another pair of templating agents may be available with RX values of approximately 140 A, and molecular volumes of around 310 A 3. I
....
I"
"..~" ~
I .~...
'I
.~ i
....~I ....... 1 '
9
!! ~IB"
....:~" ",. ...I"
I ...-.:..
.....-~" \
i~/
< ..................
........." ~.
~ I
...,.I
I
!i
..
.~I ....... .....I ....
.~i . . . . ......I ....
~.i
!
!
!
"q!ll"
"l!tl"
........ I
"~IV
".~" ",,. ~.I
I ...~..
9
~ .,.~..
!
....:.:" ",,.
....... I
i ...~,..
.,
9
'.1....
~q!P',
..,..i
!
....!
9
.....i
"q
{.::::~::;;~:::;~:::.:i..::==========================:~::::~..:::.i..::~:::::~::::~:::..~.:::~i:;;~;::;~:::.:i.:::~;::::~:;::~:::.:~
Figure 4. Poremap showing the lobed one-dimensional channel system found in zeolites with the MTT structure. Manually docked molecules illustrate possible sites available within the lobes, from top left: pyrrolidine; 2-aminoethanol; dipropylamine; and heptamethonium.
122 Plotting the principal axes of inertia for a particular template can give some indication as to which zeolite framework structures may be synthesised using that agent. The dibenzyldimethylammonium ion (DBDMA) forms at least three types of zeolite lattice (see Figure 5), the actual outcome of a preparation being dependant not only on the template shape, but also on the chemical composition of the reaction media, and the conditions under which the synthesis is performed. The DBDMA ion can therefore be considered to be a member of three distinct sets of templates. The principal axes of inertia for these templates are plotted in Figure 6; DBDMA occupies a point which lies at the intersection of the three regions of 'shape-space' relating to the structure types BEA, EUO, and MTW. The ion is accomodated in different ways in each lattice, as illustrated in Figure 5.
a
b
C
Figure 5. Three different modes of accomodation for dibenzyldimethylammonium in zeolite framework types a) BEA, b) EUO, and c) MTW. The overlap region between sets of template structures becomes very pronounced towards the origin of the RX plots. In examples such as the NON, SGT, MTN, DDR, and DOH frameworks, factors other than RX values may also need to be considered in order to differentiate between what are actually very closely related sets of templates. The small template molecules that plot near the origin can, like pyrrolidine, produce a variety of structures, depending on a range of other variables in any given synthesis. Other shape descriptors from QSAR could yet be suitable for template analysis, and although none might have the convenience characteristic of the principal axes of inertia, they
123
3
x
2.8 2.6
.,,
=// =1://,
"1= l/l/
2
1.4
RY
3 4
70 60 50 40 30 20 10 0 RX 5
80
Figure 6. Principal axes of inertia (/~) for templates forming BEA it, EUO m, and MTW (part of set) ~ framework types. DBDMA O, falls at the intersection of the three types. may provide additional structural information. Comparative Molecular Field Analysis [14'151 (CoMFA) may be used to investigate the steric and electrostatic fields which define templates. However, CoMFA requires that target molecules be aligned identically before any comparison ac be made, and therefore analyses are restricted only to very closely related sets of templating agents. It may however provide a tool which can identify the template charge characteristics necessary to produce zeolites with a certain Si / A1 ratio, or crystal morphology. It has been suggested that CoMFA be applied directly to describe the quantitative structure-activity relationships of zeolites with known catalytic properties, t141
4. CONCLUSIONS The principal axes of inertia provide a basic quantitative description of the shape of organic templating agents, and if taken into account with molecular volumes, can increase the current understanding of the influence of template structure on the structure of zeolite pore systems. These descriptors also offer an indication as to the differing manners by which various templates are incorporated into the channel system of any one zeolite, t16] The use of structure descriptors is complementary to Monte Carlo-Simulated Annealing [4'171 and, perhaps, D e N o v o methods, and could establish which shape criteria are necessary to allow rational computer assisted design of novel catalytic zeolite systems to be realised. New and improved templating agents could be sought by screening the RN values of candidate molecules, and comparing them against the known values from previously successful templates. Novel templates may also be pursued using the concept of shape and sub-shape, whereby, for instance, cheaper and smaller agents may be identified as effective sub-units of larger molecules, and vice versa. Plotting a new template upon a principal axes of inertia 'shape-space diagram' may predict which zeolite structures it might produce in addition to any
124 (more desirable) target type, and then the optimum reaction conditions necessary for its deployment may begin to be established. The authors are currently seeking to supplement the described preliminary survey by accounting for the importance of template shape in respect to other variables in zeolite synthesis, notably the electrostatic profiles of organic templates, gel chemistry and reaction conditions. A detailed chemometric or quantitative structure-property relationships (QSPR) analysis of the available data may yield information which will permit specific preparative methods to be identified for the deployment of novel templating agents.
REFERENCES
10
11
12 13 14 15 16 17
H. Gies and B. Marler, Zeolites, 12, (1992), 42. B.M. Lok, T.R. Cannan, and C.A. Messina, Zeolites, 3, (1983), 282. L.B. McCusker, Materials Science Forum, 133-136, (1993), 423. A.P. Stevens, A.M. Gorman, C.M. Freeman, and P.A. Cox, submitted to J. Chem. Soc., Faraday Trans., (November 1995). A.P. Stevens and P.A. Cox, J. Chem. Soc., Chem. Commun., (1995), 343. See, for example, "Modelling of Structure and Reactivity in Zeolites," (ed. C.R.A. Catlow), Academic Press, London, (1992). C.M. Freeman, D.W. Lewis, T.V. Harris, A.K. Cheetham, N.J. Henson, P.A. Cox, A.M. Gorman, S.M. Levine, J.M. Newsam, E. Hemandez, and C.R.A. Catlow, in "ComputerAided Molecular Design: Agrochemicals, Materials and Pharmaceuticals," (eds. C.H. Reynolds, M.K. Holloway, and H.K. Cox), ACS, Washington DC, (1995), 326. D. Livingstone, "Data Analysis for Chemists," Oxford University Press, (1995). P.M. Dean, "Molecular Foundations of Drug-Receptor Interaction," Cambridge University Press, (1987), 254. P.C. Jurs, S.L. Dixon, and L.M. Egolf, in "Chemometric Methods' in Molecular Design, Methods' and Principles in Medicinal Chemistry Volume 2," (ed. H. van de Waterbeemd), VCH, (1995), 15. A list of calculated values for the principal axes of inertia relating to the templates included in this study are available on request from the authors, together with full details of the literature source for each. Discover 3.1 program, Insight H User Guide, Version 2.3.6, Biosym Technologies Inc., San Diego, USA, (1993). Tsar version 2.02, Oxford Molecular Ltd., UK, (1993). R.D. Cramer IU, D.E. Patterson, and J.D. Bunce, J. Am. Chem. Soc., 110, (1988), 5959. K.H. Kim, in "Molecular Similarity in Drug Design," (ed. P.M. Dean), Blackie Academic and Professional, Glasgow, (1995), 291. See also R.E. Boyett, A.P. Stevens, M.G. Ford, and P.A. Cox, to be submitted to Zeolites, 1996. P.A. Cox, A.P. Stevens, L. Banting, and A.M. Gorman, in "Zeolites and Related Microporous Materials: State of the Art 1994," Studies in Surface Science and Catalysis, Vol 84, (eds. J. Weitkamp, H.G. Karge, H. Pfeifer, and W. H/51derich), Elsevier, Science B.V., (1994), 2115.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 1997 Elsevier Science B.V.
125
QUANTITATIVE ASPECTS IN'I'HE CRYSTALLIZATION OF ZEOUTES H. Lechert, T. Lindner and P. Staelin Institute of Phgsical Chemistrg, Universitg of Hamburg, Bundesstr. 45, D-20146 Hamburg Kegwords: Zeolite Crgstallization, Si/AI-ratio, crgstallization rate 1. S U M M A R Y
The Si/AI-ratio in zeolite products can be described in a wide range of batch compopositions bg a simple relation with the SiO~- and the OH-- content in the solution phase. With some simplifications this Si/A~ratio can be related to the Si/AI-ratio n and the excess alkalinitg rn in the batch. Further is shown that the rate constant of linear growth k depends on the SiO..-, the [AI(OH). ]-, and the OH-- conctentration in the solution bg a relation similar ~o the equation o4f LANGMUIR-HINSHELWOOD, showing that the formation of the surface structures tgpical for the growing zeolite is the rate determining step of the crgstallization. 2. INTRODUCTION The cr'gstallization of zeolites is still more an "art" in which experience and sometimes tricks lead to the desired results rather than well established theoretical models, connecting the wanted properties of the product and the starting parameters of the batch composition. Usuallg the solution concentrations of possible building units of different zeolite tgpes are related to these starting parameters (see e.g. CAULLET and GUTH [1] ). For the description of the batch composition the Si/AI-ratio n, the excess alkalinitg m, and the water content p are usuallg used in NaAIO 2 n ( SiO 2 m NaOH) p H 20 (1) The silicate and aluminosilicate species in the solution, which are regarded to serve as building units, are preferably studied by NMR -spectroscopg [2,3]. A second approach is the study of the crystallization kinetics. Here two ideas are discussed. One is related to the AVRAMI-theory, trying to describe the whole process of crystallization by a single function [4-6]. Often, the processes of nucleation and growth are separated. The growth can be discussed in terms of the common crystallization kinetics ( see e.g. [7,8]). The kinetics of nucleation can be described from the knowledge of the growth parameters and the particle size distribution [4]. In [9] this procedure has been used for an estimation of the size of the nuclei in nucleation gels. In this paper the Si/Al-ratio and the rate constant of linear growth of crystallizing
126
zeolites are related with the concentrations of different species in the solution phase and with the parameters n and m in Eq. 1. 3. EXPERIMENTAL The experiments have been carried out as described in our former papers [7,8]. The gels were prepared from Na- aluminate, NaOH and water glass ( d = 1.37 ). For the aluminate solution AI(OH)_ was dissolved in NaOH so that 1000 g solution contained 2.5 mol AI(OH)_ and 5 mol NaOH. The silica source was water glass with 3 273.5 g (4.6 mol) SiO 2 and 83.3 (1.3 tool) NaOH in 1000 g solution. The total concentration of the solid was chosen at 50g ( AIO - + n SiO )/1000 g H O for all ex2 periments. The general composition of the batches can 15e described ~y Eq.1. The solutions were mixed at room temperature in PE-bottles. After 1 h NaX nuclei or nucleation gel were added. Before heating to 90~ the mixture was shaken for another hour. The NaX nuclei were obtained from batches with the composition NaAIO_ 2 (SiO~ 2.4 NaOH ) 400 H~O [7,8 ], the nucleation gel from batches with NaAIO 2 7.5 ( STO2 2 NaOH ) 150 H~3::) [9,10]. The nucleation gel was aged for 5 days at room temperature before use. "l-Se products were filtered, washed, and dried. The characterization was done by XRD comparing the intensity of the (555) - reflex with that of a well crystallized zeolite. The Si/AI ratio was determined by RFA or by EDX. The solutions of the earlier experiments have been analyzed with classical chemical methods, the other by ICP-AES. Some of the samples have been studied by 29 Si and by 27AI- MAS-NMR spectroscopy. For the kinetic studies, 10 ml samples were taken from the reaction vessel which were characterized in the described way. In later experiments the crystallization was carried out in 10 ml teflon vessels which were taken from the oven after appropriate times. 4. RESULTS AND DISCUSSION From a large set of data relating the Si/AI-ratio in the products with the silicate,the aluminate and the OH- content in the solution can be seen that (Si/AI)prod = 1 + b*lSiO 2 I~o~/I OH-Isol
(2)
with b = 1.92 for faujasite and some related zeolites [10]. The concentrations in the solution can be estimated from the batch parameters n, m and p with some accuracy. The aluminate concentration in the solution is about two orders of magnitude lower than the concentration of the silicate. Therefore it can be concluded that almost all of the aluminate and a corresponding amount of Na vanishes in the gel phase.
127
For IOH-I ~oI can be obtained (3)
]OH-Isol = n * m * 5 5 . 5 / p
Assuming that after sufficient aging the Si/AI-ratio in the gel phase is nearly that of the crystallizing zeolite (Si/AI) , ~ (Si/AI) , . (4) gem proaucl the silicate concentration in the solution can be estimated by
ISiO2 Isol = [(si/AI
)batch - (Si/AI)
,]. 55.5/p =
[ n ~'(Si/AI )prod ] •55.5/p
(5)
An experimental check of Eq. 4 and also data from the literature [11 ] show, that for typical zeolite batches this assumption is fulfilled with good accuracy. With Eq.2 can then be concluded, that (Si/AI)
prod
=
n * (b + m ) /
(b + n , m )
(6)
where for the faujasites and for related zeolites b = 1.92 ~ 2 can be used.. This argumentation and especially Eq.4 is possibly no more correct for low m and high n in the batch, because of the presence of colloidal SiO 2 in the gel as well as in the solution. In these cases higher values of b may be expected. Preliminary experiments with zeolite Beta and some pentasils confirmed this. The importance of Eq.6 is that it relates directly the Si/AI ratio of the product to the parameters m and n in the batch. The reliability of Eq.6 is shown in Fig. 1 for data from [10 ] and from this work in which the solution phase has been carefully analyzed. It can be seen that Eq.6 is fulfilled with b = 2 with a surprisingly high accuracy. A further test with data from the early literature summarized in the book of BRECK [12] is demonstrated in Fig.2. At the present stage of argumentation Eq.6 has to be regarded as a more or less empirical relation. As long as the assumptions made in the derivation of Eq.6 from Eq.2 are true, the explanation of Eq.6 is connected to the explanation of Eq.2. In a preceding paper we have discussed a model for the dependency of the Si/AIratio of a crystallizing zeolite on the OH- concentration in the solution[13]. This model starts from the assumption that the S i / A I - ratio is determined at the surface of the growing zeolite. The surface consists of the groups - AI-OH ]- , - Si-OH .and Si-O-. Between the silicate groups an equilibrium can be assumed: -=Si-OH + OH- = -Si-O+ H20. (7)
128
5.0 u
I,
4.0
-i-.....L
t
0
o_
+
!
ii
V
i
! iv
i i
I I
!i
i
2.0
3.0
,i "........................
2.0
i
1.0 1.0
n9
;
(2 + m)*n/(2
5.0
n=3
a
n=4
II
n--5
o
n-6-9 9
i
4.0
1.4,1.5
9 n = 2-2.5
3.0
E
tJ)
i
v
n>10
Mordenit
+n'm)
Fig. 1 Si/AI- ratios of faujasites with batch compositions with different n and m compared with values predicted by Eq.6
+ u :3 "13 O Q..
Mordenite 9 Analcime 9 A, HS,Zh, Cancrinite
E
0
Om
o
<
0
o /
r
a
P,R,S,X,Y
-
ZSM3,Mordenite with Li
i
0
!
0
!
|
|
|I
|
|
2
(2 + m)*n/(2
|
w
4
6 +n'm)
Fig.2 Si/AI ratios in different zeolites from batch compositions
with different n and m, and different cations taken from BRECK [12] compared with the values predicted by Eq.6
129
If it is further assumed that the aluminate from the solution reacts preferablg with the = Si-O- groups via a nucleophilic substitution reaction and the silicate with the = Si-OH via a condensation reaction, for the Si/AI- ratio an equation of the kind (Si/AI)prod
=
1 + a /IOH-I
(8)
can be derived. This relation describes the Si/AI-ratio of the product onlg if the Si09-concentration in the solution is held constant. It can be seen that the model usec~ for the derivation mag be correct with some further modifications taking into account the influence of the silicate which is found experimentallg in Eq.2. Regarding that the formation of a zeolite is a preferablg kinetical phenomenon, in which the Si/AI-ratio mag be given bg some kind of steadg state of the attachment of silicate and aluminate to the surface, in the following an extended number of kinetical experiments from this and our earlier papers shall be analgzed [7,8]. In these experiments the rate constants of linear growth k have been studied. The k have been related to the concentrations of [AI ( OH )4 ] - ' S i 0 2 ' and OH- in the solution phase. In Fig.3 the rate constant of linear growth k is plotted against the ratio of IOH -I , /ISiO.. I~ I" IOH-I_ I is an estimate of the concentration of the free alkali sqi .. ~ q~ in the sotutlon, given t)y the di~erence of the total alkali content and the silicate content in the solution, because from [1 ] can be seen that in the range of alkalinities in discussion here, the silicate in the solution phase is present preferablg as NaOSi(OH) 3 . As can be seen in Fig.3, k is a linear function of I OH -Isol/ISiO.2 ] , almost independent of n if n > 4. For low ] OH -I , / ISiO_! correspono~ng~h high Si/AIratios in the products the function o ~ ' o n thisz , ~ / b e c o m e s uniform for" all n. For lower values of n, k decreases distinctlg. In this region k is proportional to I OH - Isol * ISi02 ! sol with some accuracg. Both relations can be brought into a common equation bg k
=
or"
k
=
C 9( I OH -
- I SiO2 I=o )'1 sio2]~o t ( 1 + I SiO 21 sol ) 2
C *9 I AI(OH)4 - I~ol * ISiO 2 I sol )2 ( 1 + I Si02 I~ot
(g)
(10)
130
c-
E I
O tO r"
o
"-U
o
~-
c~i
4.0
+
Si/AI = 1.4
!
, ~ d
3.0 J 2.0
i
-
1.0
aJ
........................i.....................
--'i .......
i-"
121(
',
0.0 -2.0
2.0
i
1
I
6.0
10.0
14.0
(I NaOH l-IS~O= I)/I s~o= I
9
1.5
9
2.0
a
3.0
,,
4.0
o
5.0 9 6.0-9.9
9
>
10.0
Fig. 3 Rate constant of linear growth k in dependence on the ratio
IOH-Iso~/ISi021so~ c-
4,0
E I
o ,,I,--.
tO t/} tO u
o L_
, !
3,o
I
Si/AI = 1.4
i
i i
L -T--'
i io@O
o 9
2,0 ~- .... : ........... ,.-.-~s-; .............. 1,0
t
i
I~
~
i
1
i
0,0
0,2
0,4
!
=
i i
2.0
v
3.0
+
4.0
o
5.0 9 6.0-9.9
o,o -0,2
1.5
0,6
9
>
10.0
(I NaOH I-ISiO2 I)*1 s~o= I/(] + I SiO2 I) = Fig. 4 Rate constant of linear growth k in dependence on the relation given bg Eq.g
131
because it is [AI(OH) 4 ]-sol "" l OH-J,ol over a wide range of concentrati0ns. The data corresponding with Eq.9 are demonstrated in Fig.4. It can be seen that the data are described by this equation with good accuracy. Eq.9 is together with Eq. 10 similar to a LANGMUIR-HINSHELWOOD -equation for the formation of a structure of the kind (11) - Si(OH)2 - 0 - AI (OH)2 This means that the concentration dependence of the crystallization rate can be understood by a model in which the formation of a surface structure as e.g. a fourmembered ring is a rate determining event [14]. For a decision whether the ring closure or the attachment of the silicate or aluminate may be rate determining a more detailed discussion with the more extended relations of HOUGHEN and WATSON [15] has been carried out For the attachment of aluminate as rate determining step can be written
C'.( I AI(OH)4- I~o~ - SS/(ISiO21.ot*K) )
k =
(1+
CAt
AI(OH)4 -I ~ot * cslSiO
2
Isol }2
(12)
SS is the synonym for the surface structure and K the equilibrium constant of the formation of the ring structure from neigbouring - Si(OH) and -AI(OI-i) - 3 3 groups at the surface. K can be regarded to be large taking into account the low solubility of the aluminosilicate. Eq.12 becomes different from Eq.10. It can be shown that a uniform description of the experimental data is not possible by Eq. 12. Therefore, it can be seen that the dependence of k on the concentrations in the solution phase can be described by the formation of the rings given by (11) - or possibly structures formed in a consecutive reaction - as rate determining step. From Eq.10 follows that k is for the whole range of faujasites proportional to the concentation of the aluminate in the solution. The crystallization rate should, therefore, be increased with the concentration of the aluminate.. In two separate papers [16,17] the effect of the addition of fluoride and a series of complexing agents for the aluminate was thoroughly studied. It could be seen that the crystallization rate can be appreciably increased, especially for the crystallization of Y-zeolites supporting the foregoing arguments.
5. A
C
~
~
The authors thank for the support of this work by the "Deutsche Forschungsgemeinschaft.
132
6. R E F E ~ E S 1. P. Caullet and J. L. Guth, ACS Symp Series, 398 (1989) 83. 2. G. Harvey, L. S. Dent Glasser, ACS Symposium Series, 398 (1989) 49. 3.A.T. Bell, ACS Symp. Series, 398(1989)66. 4. S.P. Zhdanov and N.N. Samulevich Proc. 5th Intern. Conf. on Zeolites L. V. C. Rees Ed., Heyden, London 1980, p. 75. 5.M. Avrami, J.Chem.Phys., 9 (1941) 177. 6. R.W.Thompson, Zeolites, 12 (1992) 680. T. H. Kacirek and H. Lechert, J. Phys. Chem. 79 (1975) 1589. 8. H.Kacirek and H. Lecher-t, J.ChemPhys. 80(1976) 1291. 9 H.Lechert, P. Staelin, M. Wrobel and U. Schimmel, Studies in Surface Science and Catalysis 84A (1994) 147. 10. H.Lechert, P. Staelin, and Ch Kuntz, Zeolites 16 (1996) 149. 11. S.P. Zhclanov, S.S. Khvoshchev, and N.N. Feoktistova, "Synthetic Zeolites", Gordon and Breach Science Publishers, New York, Philadelphia, London, Paris, Montreux,Tokyo, Melbourne, 1990. 12. D. W. Breck, "Zeolite Molecular Sieves" John Wiley, New York, 1974 13. H. Lechert, H. Kacirek, and H. Weyda, in "Molecular Sieves" M.L. Occelli and H. Robson Eds., Van Nostrand Reinhold, New York, 1992, p. 494. 14. H. Lechert, Zeolites (in press). 15. O. A. Houghen and K. M. Watson "Chemical Process Principles" Part III Wiley & Sons, New York, 1948. 16. T. Lindner and H. Lechert, Zeolites, 14 (1994) 582. 17. T. Lindner and H. Lechert, Zeolites, 16(1996) 196.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
133
A computational 'Expert System' 'approach to design synthesis routes for zeolite catalysts T. Selvam, D.N. Iyert , R.C. Deka, A. Chatterjee* and R. Vetrivel* Catalysis Division, National Chemical Laboratory, Pune-411 008, INDIA. Fax: +91-212-334761 /330233.
We have developed a knowledge based database system on zeolites for IBM-PCs operating on MS-DOS. The system contains a database of physico-chemical and structural properties of all the molecular sieves. The data could be retrieved from the database by choosing answers to questions from a menu driven sot~ware and hence no background knowledge of computers is assumed. Further, the wide experience in the synthesis of molecular sieves, particularly zeolites, ZSM-5, ZSM-11, AIPO4-5 and AIPO4-11 available in the literature are collected and conserved. An 'expert system' approach is developed to derive a set of conditions to achieve one's goal in the synthesis of zeolites. The most suitable conditions of synthesis are decided based on the published data in the literature or based on the correlations derived from the reported data. This system includes the graphical display of the powder diffraction pattern for various molecular sieve structures, as well as their mixtures. By pattern matching procedure, it is possible to identify and analyze the impurity phases and yield in the synthesis batches.
1. INTRODUCTION Molecular sieve materials which comprise zeolites, ALPOs, etc., are the single class of catalysts having maximum commercial applications. The application of zeolite catalysts has penetrated into the areas of environmental catalysis and fine chemical synthesis, in addition to petroleum and petrochemical industries. Nearly 100 molecular sieves with established structures are reported [1] and more than 200 hypothetical molecular sieve structures are predicted [2]. In proportion to their scientific and technological importance, knowledge and information on existing as well as new zeolite structures are accumulating over the years. The design of a new catalyst involves logical application of all the available information. It is becoming a difficult task to manage the available information on molecular sieves by human experts. , Present address : Dr. Reddy's Research Foundation Bollaram Road, Hyderabad 500 138, India * Present address : Tohoku National Industrial Research Institute, AIST - MITI, 4-2-1, Nigatake, Miyagino-ku, Sendai 983, Japan * Author for correspondence.
134 Earlier attempts in the direction of systematically storing and effectively utilizing the information on catalysts include: i) a data base on C~ catalytic chemistry by Ito et al [3] ii) computer aided design of catalysts for oxidation reaction using expert systems approach [4,5] and iii) expert system approach to design a catalyst [6]. Computerization of information on zeolite catalysts have also been reported and different databases concentrate on specific properties [7-10]. They contain extremely useful information as shown in Table 1. In this study, we have attempted a systematic information technology approach and an Expert System (ES) approach to computationally design the synthesis routes for zeolites. Table 1 Existing; databases containing; information on zeolitic system. Database Hardware Information Content Advantages Platform Zeofile Macintosh Physico-chemical Simulation of powder property, diffraction pattern for a crystallographic known crystal structure is information, possible. Any textual and structure and graphical information topology of all could be exported to Word materials in Ref. 1. processor files.
Reference 7, 10
Zeopak
VAX system
Powder diffraction patterns of synthetic and natural zeolites,
Identification and quantification of zeolite phases. Characterization is possible by pattern matching.
8
Zeobase
IBM-PC AT 286 and above
Crystalstructure of Entries on as many as 1300 various modifications materials are available. Xof zeolites, ray patterns and molecular models of zeolitic materials can be viewed on screen, plotted on printer or plotter.
9
2. METHOD OF APPROACH
Our approach is to develop an user-friendly software system which can aid the design of molecular sieve catalysts. The task of 'molecular sieve design' can be resolved into many smaller tasks and the smaller tasks could be completed in a step-wise manner. The smaller tasks in catalyst design are listed out as follows:
135 i) propose the list of required physico-chemical properties in a zeolite for a specific end-use, ii) screen out zeolites by searching for a known material possessing all required properties, iii) if one is available with all desired properties the search is completed successfully, which is most unlikely. Alternatively if few molecular sieve materials are available whose properties are reasonably closer but not exactly as needed, find out the ways of modifications to improve or bring it to the level of satisfaction. iv) list out the side-effects or unfavorable properties that may get introduced due to modifications and find ways of eliminating them and v) design a viable and efficient synthesis route for the zeolite proposed in step (iii), taking into considerations of the points listed in step (iv). When the above tasks are completed, the number of experiments needed to design a molecular sieve catalyst could be restricted to a limited number and many trial and error process could be minimized. As recently pointed out, systematic correlations are derived between the critical factors that influence the zeolite synthesis and the kinetics, the quality as well as the yield of the zeolites formed [11]. The availability of all information as a single source, that too in a convenient electronic media is an asset, in our own experience. The retrieval of information on any specific known molecular sieve or on all molecular sieves with specific property is straightforward with our well structured database. An inference engine using logical computer language such as PROLOG is developed to make decision from the data provided in the form of mathematical relations. Thus an efficient research tool which reduces the burden involved in the above mentioned steps in the molecular sieves catalyst design is developed. Additionally, this shall be an effective educational tool for any beginner in the-field of molecular sieves. A 'question-answer' interactive session between system and user is useful as a tutorial for novice in the field of molecular sieves.
3. APPLICATIONS The structure of the system is designed to perform three salient functions as shown in Fig. 1. The first feature provides access to a large database of physico-chemical properties and crystallographic information of all reported zeolites [1]. The second feature provides interactive access to the expert system for the synthesis of zeolites. At the end of the session, the most logical route for the synthesis of a desired zeolite structure is provided. The third feature is a graphic tool box application to simulate X-ray powder diffraction patterns for zeolite phases with different amounts and nature of purity. 3.1.
Source of information
The salient information which are incorporated in the database for different zeolites are given in Table 2. Molecular sieves can be sorted out based on specific value or a range of values of a property. For example, one or all molecular sieves having a framework density of 14.0 T/1000/I,3 or in the range 10.0 to 15.0 T/1000A 3 could be sorted out. Additionally, a combination search for molecular sieves could be performed. This allows one to choose all materials which have a desired value or range of values for multiple properties. For example it is possible to select all molecular sieves having a framework density values in the range 10.0 to 20.0; bidimensional channel architecture; small pore system and orthorhombic symmetry could
136
OPENING
MENU
| EXPERT SYSTEM
DATA B A S E
ZEOLITE- b
KNOWLEDGE F,
WISE
BASE
'ROPERTIES R-C--I'PRO~~T O y(
GRAPHICS TOOL
WISE
QUESTION -
'
INFERENCE ENGINE
PDP FOR PURE PHASES
/~A ETERM INESX ZEOLITE WITH DESIRED PROPERTIES
M INE$ 7 DAETER LOGICAL ROUTE FOR SYNTHESIS
I" ~
II~IPHASES WITH III I I M P U R I T Y
INTERACTIVE SESSION
ANSWER SESSION
/
h
INTERACTIVE SIMULATION ~ THETERMIN ES" E P HASE COMPOSITION
Figure 1. Outlook of the sot~ware
Table 2 Salient information on each molecular sieve stored in the data base General 3 letter code Expansion of the code - full name P h y s i c o - c h e m i c a l properties Structural properties Framework density (Fwd) Secondary building unit Dimensionality of the channel (Dim) Crystal symmetry (Xst) Pore size Crystal space group (Xsg) Pore dimension Unit cell dimensions Isotypic framework structure Atomic co-ordinates of unit cell Miscellaneous
Catalytic properties Dimension of reactant molecules Dimension of template molecules Template, synthesis conditions and reference
137 Table 3 A typical sample screen is shown for a combination search performed. INPUT SELECTION Data Entr~ Menu
I SearchMenu ] Reports Exit IF i
[,Zeolite
I
Starting Material Exit Zeolite
Property [ Combination Properties
I
Exit Framework Density Between : 10.0 and 20.0 Dimensionality 92
Pore Size Crystal Structure
: SP : ORT
OUTPUT PRODUCED Zeolite
Fwd
Dim
Xst
APC APD ATT MON
18.00
2
19.80
2
16.70 18.10
2 2
ORTHORIIOM ORTHORHOM ORTHORHOM ORTHORHOM
Total
Xsg Pbca
Pca21 P212121 Fdd2
4 zeolites
be sorted out as shown in Table 3. A boolean search with 'and', 'or' and'not' options can be performed on zeolite names, zeolite structure codes, framework density, keywords, space group, crystal system, unit cell volume, catalytic performance and authors of the work. The output always appears on the screen and there is option to store the information to the hard disk of the computer as a file for future reference or to output as a hard copy in the printer for the usage on a WYGlWYS ( what you get is what you see) basis. There is always a hot-key (F l) help facility i.e., whenever F 1 key is pressed, a help information regarding the menu items on the screen are displayed.
138 A list of reactions catalyzed by a certain zeolite is also included. The dimensions of many hydrocarbon reactant molecules are part of the data base. Hence it is possible to get a first hand information above the suitability of a molecular sieve to adsorb reactant molecules. Sorption capacity of molecular sieves from experimental reports for various molecules are also added.
3.2. Designing a synthesis route by ES approach Nearly 75 different conditions of synthesis for ZSM-5 [12] and 25 different conditions of synthesis for each of ZSM-11, AIPO4-5 and AIPO4-11 were collected from the literature. These different "conditions" include the variations in the templating organic molecule, temperature, time, static or stirring, composition and source of hydrogel as well as pH. Templates were arranged in the order of descending efficiency. Inverse linear correlations were observed between temperature and time of crystallization as well as between efficiency of the template and time of crystallization. The dependence of time of crystallization on the above mentioned conditions were plotted and fitted into suitable mathematical relations. The system initially starts by enquiring the user for the final "output" of preferred phase, yield, crystallinity and morphology. The database is searched to see if these requirements could be met by match-making with one of the existing reports in the literature. In the absence of a synthesis route in the reported literature, the system chooses the conditions from the mathematical relations already established. Here, it is assumed that the data published in the literature are correct and they could be extrapolated or interpolated to valid regions, where there are gaps in the literature. The conditions are varied within a predefined range, so that finally all conditions fit into the mathematical relations between the "conditions" and "output", within an error count of 10%. The system registers an error message, in case the required output cannot be achieved within 10% error of variation in conditions. Thus the system chooses optimal conditions for the synthesis to satisfy the requirement of the user. The system solves problems which are often poorly defined or understood. At each decision making point, the system starts by providing an introductory note about the conditions being varied as well as typical case studies which are available in the literature.
3.3. Analysis of phase purity in synthesized samples Simulated powder diffraction patterns (PDP) of all the molecular sieve materials are presented in the form of a graphic display or in the form of a table of 20 and relative intensity. It is possible to simulate PDP of mixture of more than one zeolite. When PDP of more than one structure is displayed, the pattern for each structure is displayed in different color. This facility is useful to analyze the phase purity of any synthesized sample. For example, it is well known that ZSM-11 phase occurs as impurity while synthesizing ZSM-5 phase and vice-versa. In Fig.2a and 2b, the PDP of ZSM-5 and ZSM-11 are shown, respectively. Fig.2c shows the PDP for a 50:50 mixture of ZSM-5:ZSM-11, which is a typical example. If the PDP of synthesized sample matches with Fig.2c, the phase concentration could be inferred. Similarly PDP can be simulated for different proportions of the individual component, till it matches with the experimentally observed pattern. As an another typical example, the PDP of AIPO45, AIPO4-11 and the simulated PDP for 75:25 mixture of AIPO4-5:AIPO4-11 are shown in Figs. 3a, 3b, and 3c, respectively. If a sample obtained from AIPO4-5 synthesis batch showed a pattern as in Fig.3c instead of Fig.3a, then 25% yield of A1PO4-11 could be inferred. Thus using this facility, the impurity phases and the selectivity in the synthesis could be identified.
28
28
28
Figure 2. The PDP generated by the system for ZSM-5 (a), ZSM-11 @) and 5 0 5 0 ZSM-5:ZSM-11 100. F
- 100
100.
(a 1
-
80
-
-
80 60
60
-
1
w40-
40
40
-
320-
20
20
-
Ero E60
I
(c 1
W
a
t
0
1
5
I
10
L
IS 28
a
20
1L
25
30
0
5
10
IS 28
20
2530
0
I
1
5
10
Figure 3. The PDP generated by the system for AlP04-5 (a), M 0 4 - 1 I (b) and 75:25 ~ 0 4 - 5 : M 0 4 - 1 1
I
I l A
IS 2 0 2 5 28
30
140 4. SUMMARY Molecular sieves literature today is vast and versatile. Although one may remember that an information is available in the literature, it becomes a hard or sometimes impossible task to search and retrieve that information from the books and journals. However, one should recognize that the 'information science' has benefited largely by the advent of powerful computers and efficient software packages. Desktop personal computers which have attained the status of'essential equipment' of any researcher are good enough to handle vast amount of information efficiently. We felt that one massive attempt to collect all the information, classify and store them systematically as well as to create a 'user-friendly system' to retrieve will help the whole molecular sieve research community. The database is further upgraded as an ES to design a logical route for the synthesis of zeolite. The routes are decided from either well documented synthesis procedures or from correlations derived from the reported data. Thus the feasibility of ES approach has been tested and shown as powerful tool for computer aided design of catalysts.
ACKNOWLEDGMENTS The authors (TS, RCD & AC) thank UGC and CSIR for financial support in the form of Research Fellowships. We thank Dr. S. Krishnan and Dr. P. Ratnasamy for initiating the building up of the database reported here. We acknowledge the programming expertness provided by S. Mani, S. Hajamis, S. Ganorkar and V. Dhayagude. Many people in Catalysis Division, National Chemical Laboratory actually used the system in its primitive stage and suggested improvements which made it user-friendly. The work was partly funded by UNDP.
REFERENCES
1. W.M. Meier and D.H. Olson, in: 'Atlas of zeolite structure types', Butterworth Heinmann, London 1992. 2. J.V. Smith, Chem. Rev., 88 (1988) 149. 3. T. Ito, H. Hamada, Y. Kintaichi and M. Sasaki, Catal. Today 10 (1991) 223. 4. S. Kito, T. Hattori and Y: Murakami, Appl. Catal., 48 (1989) 107. 5. T. Hattori, H. Niwa, A. Satsuma, S. Kito and Y. Murakami, Appl. Catal., 50 (1989) L 11 6. T. Hattori and S. Kito, Catal. Today 10 (1991) 213. 7. J.M. Newsam and M.M.J. Treaey, 9th Int. Zeolite Conf., Extended Abstracts and Program, No.RP 193 (1992). 8. D.K. Smith, S.Q. Hoyle and G.G. Johnson, Jr., 9th Int. Zeolite Conf., Extended Abstracts and Program, No.RP 192 (1992) 9. W.H. Baur and R.X. Fischer, 9th Int. Zeolite Conf., Extended Abstracts and Program, No.RP 216 (1992). 10. J.M. Newsam and M.M.J. Treaty, Zeolites 13 (1993) 183. 11. E.J.P. Feijen, J.A. Martens and P.A. Jacobs, Stud. Surface Sr Catal., 84A, 1 (1994). 12. A. Chatterjee and R. Vetfivd, J. Chem. Sor Faraday Trans., 91 (1995) 4313.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
141
A new method for enhancing zeolite crystallization by using oxyacids / salts of group VA and VIIA elements as promoters Asim Bhaumik, A.A.Belhekar and Rajiv Kumar Catalysis Division, National Chemical Laboratory, Pune - 411 008, INDIA. ~ A novel and general method for highly efficient, fast synthesis (with 4-6 fold increase) of zeolite and related materials has been developed using a new concept of addition of some promoters (oxy anions like C104, PO43, AsO43, C103,etc in the form of salt or acid). The materials
produced using promoters exhibit similar, if not better, yield, crystallinity, morphology and catalytic properties compared to those obtained by conventional method. 1. INTRODUCTION Microporous, crystalline alumino- or metallo-silicate molecular sieves / zeolites [1-4] exhibit unique catalytic, adsorption and ion-exchange (viz. as detergent builders) properties. Zeolites are largely used as catalyst in various chemical, petroleum refining, petrochemical, bulk chemical and fine chemical processes [4-10]. Although, the nature of surface and catalytic properties of zeolites and related materials is relatively better understood, their synthesis continues to be intriguing and challenging. Zeolites are generally synthesised hydrothermally from an alkaline aluminosilicate reaction mixture which may or may not contain organic guest molecule (template), at autogenous pressure for few days to few weeks time. Inui [ 11 ] has pointed out various drawbacks of long crystallization time (few days or more) extensive labor coupled with delays and expense, low reproducibility and formation of larger crystals with inhomogeneous particle size distribution mainly because of secondary crystallization. However, the optimisation of recipes for each structure is done on case to case basis. Hence, ever increasing efforts are going on to reduce the synthesis time of these materials and thus to save energy and time. Now, we report, for the first time, a general method using some promoters (like C104, PO43, AsO43, C103", BrO 3" etc. in the form of acids or their Na/K salts) for highly efficient, fast
1 AB thanks CSIR, New Delhi for granting a senior research fellowship.
142 synthesis (with 4-6 fold or more increase) of zeolite and related materials with similar, if not better, yield, crystallinity and catalytic properties compared to those obtained by conventional method. A variety of zeolite structures representing small (NU-1 & FER), medium (ZSM-5 & ZSM-48) and large (Beta & ZSM-12) pore zeolites as well as aluminous / low silica (Si/A1 = 1-5, e.g. zeolite Y) and silicious / high silica (Si/A1 > 5: such as ZSM-5, ZSM-12, Beta etc.) molecular sieves have been chosen as representatives to demonstrate the generality and wide applicability of our present method.
2. EXPERIMENTAL All synthesis experiments were carded out in 200 ml capacity stainless steel autoclaves with teflon coatings under static conditions. In a typical synthesis, silica source was stirred with required amount of template and alkali dissolved in water for 1 h. Then the aluminium source (NaA102 for most of the cases) taken in water was added into it. Finally required amount of promoter (added in the form of oxyacid or their sodium / potassium salt of their corresponding oxyanions) taken in the rest amount of water was added slowly to the stirring gel. Stirring was continued for another 1 h and then the resulting gel was autoclaved. Na § / SiO2 molar ratio was kept constant for a particular zeolite by adding appropriate amount of NaC1. Gel compositions in terms of moles of oxides are given in Table 1" Table 1" Starting molar gel compositions of various zeolites Zeolite
Molar gel composition
NU-1
40
S i O 2 " A1203 " 5.0
FER
60
S i O 2 9A1203 "
ZSM-5
40
S i O 2 " A1203 " 5.0
ZSM-48
90
S i O 2 " A1203 " 9 . 0 N a 2 0
pH
Na20 " 10 (TMA)20 91000
H20"
18 N a 2 0 " 7.5 Pyrrolidine 92400 Na20" 5 (TPA)20 91200 9 15
DIQ-6 92700
12.2 _+0.2
H 2 0 " 6P
12.0 _+0.2
4P
10.8 _+0.2
H20"
n20"
4P
9P
11.6 _+0.2
ZSM-12
120
Beta
30SIO2 9A1203 "Na20 " 0.5K20 97.5(TEA)20 9600H20 93P
12.5 _+0.2
Y
9SiO 2 9A1203:4 Na20" 270 H20 9P
13.4 _+0.2
SiO 2 " AI203 " l0 Na20"
12 DIQ-6 " 3600
H20 "
12P
10.8 _+0.2
Where P = promoter chosen from HC104, NaCIO 4, H3PO 4, NaH2PO 4, Na2HPO4, Na3PO4, Na2HAsO4; TEA = tetra ethyl ammonium, TPA = tetra propyl ammonium, TMA= tetramethyl ammonium, DIQ-6 = hexamethylene bis (benzyl dimethyl ammonium), P =
C 1 0 4 , P O 4 3 , AsO43-
143 or none. The crystallisation temp (~
was = 170 (NU- 1, ZSM-48), 160 (FER, MFI, MTW) and
140 (BEA). In case of zeolite Y the standard seeding procedure reported by Ratnasamy et al.[ 12] was followed. 3. RESULTS AND DISCUSSION In Table 2,effect of various promoters used in the synthesis of different zeolite structures is shown. The use of small amount of promoters signigicantly enhances the overall crystallisation process in the order : C10 4- > PO43 > AsO43- >> none, independent of structures. Some stabilising effect of certain neutral sodium salts of some anions (e.g. NaC1, NaNO 3, Na2SO 4, NaC103 etc.) during hydrothermal transformation of kaolinite into sodalite and cancrinite has been observed [ 13] where the inclusion of these salts in the sodalite / cancrinite structure was found to be the main cause of stabilising a particular phase. In the present case of direct synthesis no such inclusion of promoters (anions or their salts) in crystalline molecular sieves was obtained. Table 2: Effect of various promoters on zeolite synthesis Zeolite
Cryst.
Si/AI
Crystallization time, h
Temp.~
(solid) a
CIO 4"
PO43"
msO43"
None
NU- 1
170
17-19
28.0
30.0
36.0
120.0
FER
160
10-15
18.0
26.0
26.0
60.0
ZSM-5
160
15-17
6.0
8.0
12.5
36.0
ZSM-48
170
30-38
40.0
44.0
40.0
108.0
ZSM- 12
160
45-50
36.0
40.0
42.0
132.0
Beta
140
12-14
30.0
32.0
36.0
156.0
Y
100
2.4-2.8
4.0
4.0
5.0
11.0
a: Obtained by chemical analysis of various zeolites using different promoters In Fig. 1, the crystallinity of zeolite Y (curves x and y) and ZSM-5 (curves a-d) is plotted against their corresponding crystallization time. The synthesis time was considerably reduced by the addition of the promoters in both the cases. However, in the case of zeolite Y, not only the crystallization rate but also the stability of fully crystalline material in the mother liquor was found to be more in the presence of a promoter (PO43-). While, following the conventional / standard method (without using promoter) zeolite P, a common impurity in Y synthesis [12], was detected immediately after 30 - 60 min. of the complete formation of Y (curve y, Fig. 1), in our method (curve x, Fig. 1) zeolite P was not observed even after 2 hours of the complete crystallization of zeolite Y. It is again clear from Fig. 1 that under otherwise same synthesis
144 conditions, the presence of promoters enhances the nucleation and crystallisation in the order: ClO 4" > PO4 3" > AsO4 3" >> none. The polarisability of the central element of the promoter (i.e.
charge / radius, Z/r value) also decreases in the same order. Further, from the nature of crystallisation curves (a-c vis-a-vis d in Fig 1), it can be inferred that the presence of promoters enhances the process of both nucleation and crystallisation.
lOOt
.~ 80-
w~'='e=w~n~=~J
,'
!
X
a
,,~r[
b
I iJY
I
I
>"
I
I
_~60-
I
I
i
I
Z
"J
I
I
"J 4 0 "
t
I
j=
I
l
U')
-/,'
-
l
I
,
'
I
~ 2O-
I !I
, '
/
4
I'
12
16
"
CRYSTALLIZATION
I
I
5
TIME , h
Fig. 1" Crystallization kinetics of zeolite Y (curve x with Na3PO4 and y with no promoter, arrow indicates the appearance of zeolite P) and ZSM-5 (curves a,b,c & d represent the use of HC104, H3PO4, Na2HAsO4 and none, respectively as promoter). For gel composition see Table 1. After having acertained the utility of various promoters, in zeolite crystallisation, it was thought worthwhile to study the effect of concentration of a particular promoter on a particular zeolite structure. NaH2PO 4 and ZSM-5 were chosen as representative. It was found that with
145 increasing the amount of promoter, the crystallisation time decreases upto Si / promoter molar ratio = 5. By still increasing the amount of promoter no further enhancement in crystallisation was observed (Table 3). Table 3: Effect of phosphate promoter concentrations on crystallisation of ZSM-5 T = 160 ~
gel composition is given in Table 1.
Si / Promoter molar ratio
Cryst. time, h a
oo
20
10
5
2.5
40
12.5
8.0
7.0
6.5
a: Time taken for obtaining fully cryStalline material, calculated from crystallisation kinetic curves
Hence, above mentioned data clearly demonstrate that a considerable increase in the nucleation and crystallisation processes of various zeolites can be achieved by adding a small amount of certain oxyacids (or their salts) of group V and VII A elements. After achieving the goal of faster synthesis of zeolites, next obvious question is to varify the quality of these materials. All samples were thoroughly characterised through XRD, SEM, EDX and weight chemical analysis. It is pertinent to mention that in all the cases comparable or better crystallinity and yield along with better uniformity of particle size distribution was obtained with the use of promoters over that prepared in the absence of promoter. The scanning electron micrographs of zeolite Y (Fig.2, a and b) and ZSM-5 (Fig.2, c and d) taken as representative, exhibited that the crystallite size of the samples synthesised in the presence of promoter (e.g. PO43, a and c) vis-a-vis its absence (b and d) is smaller along with better uniformity of particle size distribution. The crystallite size of zeolite Y was 0.6 to 0.8 Ixm and 0.8 - 1.5 l.tm in the presence and absence of Na2HPO4 respectively. Corresponding values for ZSM-5 were 0.8 - 1.0 ~tm and 1.0 - 2.0 ktm, respectively in the presence and absence of promoter. Same observations are obtained for other topologies also. Smaller and uniform crystallites size distribution indicates the absence of secondary crystallisation. When both nucleation and crystallisation processes are quite fast, the secondary crystallisation is expected to be eliminated or suppressed. The n-hexane cracking reaction was carried out over H form of ZSM-5 samples represented by Fig.2C and Fig.2d. The value of moles of n-hexane converted
146 per mole of A1 per h was 18.0 and 17.2 respectively for H-ZSM-5 samples synthesised in the presence and absence of promoter (T = 623 K) clearly suggesting that the material synthesised with promoters is quite comparable, if not better, in quality.
"'7
r
Fig.2: SEM photograph of zeolite Y ( a: with and b: without promoter, PO43-) and ZSM-5 (c: with and d: without promoter, PO43-) One of the most fundamental basis of the hydrothermal synthesis of zeolites is the mineralising property of water, which is greatly assisted by free OH concentration in the solution/gel. Apart from this basic requirement of mineralisability, other factors like, Si/A1 ratio, pH, aging at low temperature, crystallisation temperature and time etc. influence the type and quality of the crystalline material in rather specific ways. For example, in the crystallization of aluminous zeolites (Si/A1 = 1-5) the synthesis becomes faster with decreasing Si/A1 ratio while for high silica/silicious molecular sieves (Si/A1 > 5) the reverse is true [13-15]. Further, the range of
147 synthesis temperature for low and high silica zeolites is 80-120~ and 120-200~
respectively.
Similarly, organic bases (templates) play particularly significant role only in the synthesis of high silica zeolites [ 13-15]. However in our present method of using oxyacids / oxysalts of Gr VA and VIIA as promoters the enhancement in nucleation and crystallization is observed for all aluminosilicates zeolites independent of silica alumina ratio, pore size of the structures and temperatures of the synthesis. Although, the role of the promoters at mechanistic level is not clear, a direct correlation is found between Z / r of the central cation of the promoter with the decrease in crystallisation time. 4.
CONCLUSIONS The addition of small amount of some oxyacids (or their Na / K salts) of group V and VII
A elements (like C104, PO43", AsO43", C10 3- etc.) significantly promotes the nucleation and crystallisation of zeolites. Further, this method is applicable to all types of low, medium and large pore zeolites. Nearly 4-6 fold reduction in crystallision time could be achieved in all the cases. The quality (crystallinity, morphology, catalytic activity) of the samples obtained using promoters was comparable, if not better, than those synthesised by standard recipies without using any promoter. Promoters with more polarisability are more effective in enhancing the crystallisation. REFERENCES 1.
D.W.Breck,"Zeolite Molecular Sieves", Weley, New York, 1974.
2.
R.M.Barrer, "Hydrothermal Chemistry of Zeolites", Academic Press, NewYork, 1982.
3.
R.Szostak, "Molecular Sieves : Principle of Synthesis and Identification" Van Nostrand, Reinhold, New York, 1989. H.G.Karge, and J.Weitkamp, (Eds.), "Zeolites as Catalysis, Sorbents and Detergent Builders : Applications and Innovations," Elsevier, Amsterdam, 1989.
4. 5.
W.Holderich, M.Messe, and F.Naumann, Angew.Chem.Int.Ed.Engl. 27 (1988) 226.
6.
P.B.Venuto, Microporous Materials 2 (1994) 297.
7.
P.Kumar, R.Kumar and B.Pandey, Synlett. (1995) 289.
8.
A.Bhaumik and R.Kumar, J.Chem.Soc.Chem.Commun. (1995) 349.
9.
P.G.Schultz, Angew.Chem.Int.Ed.Engl. 28 (1989) 1283.
10.
M.E.Davis, Acc.Chem.Res. 26 (1993) 111.
11.
T.Inui, in "Zeolite Synthesis" (M.L.Occelli & H.E.Robson, Eds.) ACS Symp. Ser. 398, Am.Chem.Soc., Washington, D.C., 1989, ch.33, pp. 479-492.
12.
P.Ratnasamy, A.N.Kotasthane, V.P.Shiralkar, A.Thangaraj and S.Ganapathy, in "Zeolite Synthesis" (M.L.Occelli & H.E.Robson, Eds.) ACS Symp. Ser. 398, Am.Chem.Soc., Washington, D.C., 1989, ch.28, pp. 405-419.
148 13.
R.M.Barrer, in "Zeolites : Synthesis, Structure, Technology and Application," (B.Drzaj, S.Hocevar and S.Pejovnik, Eds.), Elsevier, Amsterdam, 1985, pp 1-26.
14.
P.A.Jacobs and J.A.Martens, Stud.Surf.Sci.Catal. 33 (1987) 58.
15.
J.S.Reddy, R.Kumar and S.M.Sciscery, J.Catal. 145 (1994) 73.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
149
The influence of mixed organic additives on the zeolites A and X crystal growth V. Petranovskii', Y. Kiy0zumib, N. Kikuchib, H. Hayamisub, Y. Sugi~, F. Mizukamib "Institute of Physics, UNAM, Ensenada, B.C. 22800 Mexico" bNational Institute for Materials and Chemical Research, AIST, Tsulmba, Ibarald 305, Japan
~
University, Cfifu,~01-11 Japan
The state of Al in the initial solutions for gel preparation is found to be important for the results of zeolite synthesis. Polynuclear complex of AI with chemical shift 8 = 57 ppm in the 27AI NMR spectra influences significantly the size and the shape of NaA and NaX crystals. The concentration of this complex depends on the composition of organic additives. 1. INTRODUCTION Zeolites have wide applications in diverse areas. Nevertheless, the mechanism of their growth is not completely clear [1]. A model that includes "secondary building units" (SBU) packing was suggested [2]. The problem of this model is to explain formation of these SBU from initial compounds. Another question is connected with the role of organic molecules in the zeolite synthesis. Organic compounds are frequently used as templates for zeolite growth [3, 4]. Usually it is supposed that the organic molecules direct crystal structures as space-filling agents. Joining these two models, a "can-and-cement" model of nucleation in zeolite synthesis was developed [5]. The formation of inorganic-organic composite structures was proposed as the explanation of the mechanism directing the structure [6, 7]. Chamell [8] found that the addition of triethanolamine (TEA) in the reaction mixture resulted in the growth of large single crystals of zeolites A and X. TEA molecules are not included in their crystals during the growth process. Hence TEA can not be the real template. It plays the role of a complex forming ligand. Only the polynuclear complex of tetrahedral surrounded Al with the chemical shift 8 = 62.6 ppm in the r~Al NMR spectra was detected in the initial solution [9, 10]. Such complexes (for example, similar to alumoxanes [11 ] or to well-known silicate ions [SisO-x]s" [12]) can be the prototypes of SBU. The aging of the initial solutions increases the size of NaX single crystals from 0.15 mm [8] to 0.25 mm [13]. The small concentration (less than 1%) of a new complex of AI with 8 = 57 ppm appears in the process of aging [10]. The same complex was found to be formed in the Al containing solutions in the presence of diethanolamine (DEA) or diisopropanolamine (DIPA), but other AI complexes were different [14].
On leavingfrom A.F. IoffePhysicalTechnical Institute, RAS, Saint Petersburg, 194021,Russia
150 Transformation of the shape of NaA crystals was observed in the case of their growth in DEA- or DIPA-containing gels. The reason for the shape change can be the variation of the structure of different aluminosilicate ions (potential SBU) in the presence of unlike ligands [ 14]. On the base of the data described above it is possible to expect that the simultaneous addition of di- and trialkylamines to the solution will lead to the generation of two complexes (with 8 -- 62.6 ppm and 6 = 57 ppm) at the same time. A variation of the ratio of organic additives can change the relative concentration of different complexes of aluminum in the solution and thus controls the results of synthesis. The aim of this work is to investigate the influence of the composition of organic additives on the process of crystal growth ofzeolites A and X. 2. EXPERIMENTAL SECTION
2.1. Preparation of solutions Sodium aluminate and sodium metasilicate ermeahydrate were used. The solutions with the compositions 0.42 mol NaAIO2 + 0.95 mol TEA + 55.51 mol H20 for NaX synthesis, 0.84 mol NaAIO2 + 0.95 mol TEA + 55.51 mol H20 for NaA synthesis and 0.44 mol Na2SiO3 + 0.95 mol TEA + 55.51 mol H20 for both cases were prepared following the procedure described by Charnell [8]. TEA was replaced in these solutions by the equivalent amount of DEA, DIPA or triisopropanolamine (TIPA). The concentration of dialkylamine (DEA or DIPA) in mixture was chosen to save total number of - - R - - O H groups. For that reason their molar concentration was half as much again as the concentration of TEA or TIPA. Mixtures of additives ( T I P A - DIPA, TIPA - DEA, T E A - DIPA, T E A - DEA) that contain 0%, 50%, 80%, 90%, 98% and 100% of NHR2 were selected to perform the zeolite synthesis. Analytical grade reagents (produced by Wako Pure Chemical Industries Ltd., Japan) were used. 2.2. 27A! NMR spectra Measurements of 27A1 NMR spectra for clear aluminate solutions were carried out on a JEOL GSH-200 spectrometer, operating at 51.90 Mt-k, using a 10 mm probe tube. The observations of 2~AI chemical shiRs were quoted relative to AI(I-I20)63+ (8 = 0 ppm). The references were placed in capillaries; the last ones were coaxially inserted in the NMR tubes. The measurements were done with a 90 ~ pulse of length 28.0 I~s, 256 scans. Spectra were recorded at 293 K. 2.3. Zeolites synthesis and samples examination The gels were prepared using TEA-, TIPA-, DEA- and DIPA-containing solutions, indicated above. The same silicate solutions in combination with different aluminate solutions were used for synthesis of NaA and NaX zeolites. Equal amounts of silicate and aluminate solutions were mixed at room temperature. The crystallization process was held at 75 ~ at static conditions. The size and shape of zeolite single crystals were detected with an optical microscope Olympus B061 and a scanning electron microscope Hitachi S-800.
151 3. RESULTS AND DISCUSSION
3.1. Influence of additive nature on the aluminum complexes in the solutions Only the monomer four-coordinated ions AI(OH)4" exist in the clear aluminate solution in the lack of any organic additives (Fig. 1, a). The chemical shift of AI in this compound is equal to 79.8 ppm. Addition of tri-substituted amines (TEA or TIPA) to the solution results in almost complete disappearance of the monomer ions. Simultaneously the polynuclear complex with 8 = 62.6 ppm appears (Table 1, Fig. 1, e, f). In the presence of DEA or DIPA the ion AI(OI-I)4" is kept in the solutions side by side with a new complex with 8 - 57 ppm (Fig. 1, c, d). The concentration of the last complex is small (Table 1). This is the same complex that was found for aged solutions [10]. Table 1 Relative intensity of different peaks in 27A1 NMR spectra for initial solutions with changed organic additives. Intensity of peaks (%) with 8:
Compounds
79.8 ppm
62.6 ppm
57 ppm
< 1
> 99
< 1"
< 1
> 99
-
95
-
5
90
-
10
100
-
-
2-Diethylaminoethanol (C2Hs)2NCH2CH2OH Tds(Hydroxymethyl)aminomethan
100
-
-
100
-
-
Triethylamine
100
-
-
2,2',2" =Nitrilotriethylamine
100
-
-
N(CH2CH2NH2)3 3,3',3"'-Nitrilotdpropiorfic N(CH2CH2COOI--I)3
100
-
-
100
-
-
Triethanolamine (TEA) N(CH2CH2OH)3 Triisopropanolamine (TIPA) Diethanolamine (DEA)
[CH3CH(OH)CH2]3N
HN(CH2CH2OH)2 Diisopropanolamine (DIPA) [CH3CH(OH)CH2]2NH Monoethanolamine (MEA)
H2NCH2CH2OH
(HOCH2)3CNH2 (C2Hs)3N
Nitrilotdacetic acid ~
acid ~r
N(CH2COOH)3 Glycine ~ 100 H2NCH2COOH Nitrilotds~ethylenephosphonic Acid) ~ 100 N(CH2POaH2)a *For aged solution The acids were neutrahzed by NaOH, and corresponding sodium salts were used '~
~
9
~
-
152 An aluminum ion interacts with TEA through its alcohol termination. The complex of AI with 5 = 62.6 ppm contains aluminum as ~AI--O---AI-- bridges only [9]. Moreover it is interesting that the number of identical alkyl groups connected with a nitrogen atom influences so significantly the structure of AI complexes in the solutions (see Fig. 1, b, c, e). Specifically, monodentate ligand MEA can not form polynuclear complexes of AI. Bidentate ligands, such as DEA or DIPA, form complex with 5 = 57 ppm as well as monomer AI(OH)g. Tridentate ligands (TEA or TIPA) convert all AI in the solution into the polynuclear complex with 5 = 62.6 ppm.
23 __....~ ~
11
C
j |
9'0"
23
a
'7'0'''50
!
: - _
s
ppm
9
9'0' ' '70
I
a
i
l
1
.
'
5'0 ppm
.
90'' 70
1
23 9b"
'7b"
b "5o' ppm"
_ilL_2& 9'0''''70''
3 i
I
'
i
I
'
50 ppm
3
d
'50''ppm"
,,,
90'' ' '70'' '5'0''ppm'
Figure 1.2~AI NMR spectra of the solutions for NaA synthesis: a - without organic additives; with addition of: b - MEA; c - DEA; d - DIPA; e - TEA; f - TIPA. Concentrations of additives are as described in "Experimental". Not only the number of the alkyl groups is important, but also their nature. Consideration of the data, summarized in Table 1, results in the conclusion that only in the case of two or three - - C - - C - - O H groups bonded to a nitrogen atom, does the aluminum form the polynuclear complexes. For example, in contrast to TEA, 2-diethylaminoethanol and triethylamine do not form any complexes. The same is correct for tris(hydroxymethyl)aminomethan that contains three alcohol groups, but they are not so flexibly connected with a nitrogen atom as those ones in TEA. Most likely, the structure of the complexes of AI with tri-substituted amines is similar to atranes [15] or pro-atranes [16]. However, substitution of oxygen by nitrogen (in the case of 2,2',2"-nitrilotriethylamine) leads to the disappearance of any form of the aluminum polynuclear complexes.
153 Results of interaction depend also on the nature of groups that substitute for the hydrogen atoms in the alkyl radical. Methyl-substituted derivatives (DIPA and TIPA) produce the same complexes (Fig. 1, c, d and e, f respectively). There are only the ions of monomer AI(OH)4" in the clear solutions with additives, which content carboxyl groups (see Table 1). Aluminate solutions with low Na20/AI203 ratio are usually unstable. An alumina precipitate appears after keeping them for several days at room temperature. The TEA containing solution was stable under the same conditions for at least several years. The structure of aluminum - TEA complex is still not clear. TEA influences significantly the chemistry of aluminum in the solutions. Thus, during the preparation of alumina from gels with different additives, only a gel synthesized with TEA remains amorphous up to 650 ~ [17]. It was supposed that TEA plays the role of a nucleation suppressant during the zeolite synthesis [ 18]. Probably all these phenomena are connected with the properties of the complex with 8 = 62.6 ppm. TIPA-, DIPA- and DEA-containing aluminate solutions were stable also. In contrast, the precipitates appeared after several days of storage for all other solutions (see Table 1). 3.2. Influence of additive mixtures on aluminum complexes in the solutions The simultaneous addition of di- and trialkylamines to the solution decreases the monomer ion concentration and increases the concentration of both complexes (with 8 = 62.6 ppm and 8 - 57 ppm). Synergism of their action is observed. Half amount of TEA in the presence of DEA or DIPA connect all AI in the complex with 8 - 62.6 ppm (see Fig. 2, a and Fig. 3, a).
'"|
90
9
it''
.'
k'
70
"-"
" 5'0
l~pm
Figure 2. 27A1NMR spectra of solutions for NaA synthesis with mixed TEA - DEA additive: a - 50% and b - 90% of DEA.
:i
90
-
u
10
9
|
.
|
50
,
~
9
___~
ppm
Figure 3.27A1 ~ spectra of solutions for NaA synthesis with mixed TEA - DIPA additive: a- 50% and b - 90% of DIPA.
3.3. Influence of additive mixtures on the zeolite A and X growth Variations of crystal size during zeolite growth in bath with mixed additives were investigated. Results are Summarized in Table 2 and in Fig. 4. Different dependencies were found for growth of NaA and NaX zeolites.
154 Table 2. Size of zeolite crystals grown in the presence of mixture of additives. Zeolite type
~ e
Crystal size, tim, for NHR2 concentration, % 50 80 90 98
composition
0
NaA
TEA + DEA TEA + DIPA TIPA + DEA TIPA + DIPA
24 24 16 16
28 26 21 21
37 29 27 23
32 20 29 24
47 38 23 15
39 33 22 19
NaX
TEA + DEA TEA + DIPA TIPA + DEA TIPA + DIPA
26 26 22 22
45 35 39 33
27 20 31 17
28 21 31 19
41 30 44 28
68 59 68 59
100
70
b 40 i
10
I
g
40 10 0
40
80
0
40
80
0
th 40
80
O
t 40
80
Figure 4. Dependencies of crystal size (ttm) on additive composition (% of NHR2 in mixture NR3 - NHR2) for NaA (a - d) and NaX (e - h) zeolites: a, e - TEA - DEA; b, f - TEA - DIPA; c, g - TIPA- DEA; d, h - TIPA- DIPA. For NaA zeolite the concentration dependencies of the crystal size go through a maximum when NHR2 concentration changes. Positions of these maxima depend on the nature of NR3. For TEA and TIPA they correspond approximately 98% and 80% of NHR2 in the mixture, respectively (Table 2, Fig. 4, a - d). For NaX zeolite these dependencies also have wellpronounced maxima for the 1:1 ratio of additives. Nevertheless the biggest crystals were grown in the case of pure N t ~ 2 additives (Table 2, Fig. 4, e - 11). In the all cases TEA and DEA show better results than more bulky TIPA and DIPA, both unmixed and in mixtures. Common features of these dependencies confirm that, for the results of the synthesis, the chemical state of framework components in the solutions is more important than the origin of the individual organic compounds. The chemical shift 8 = 57 ppm is known for solid state MAS ZTAlNMR spectra of the solid phase of gels and zeolites A and X [19]. Thus the action of dialkylamine changes the state of AI in the solutions to that state found in the zeolite crystal
155 lattices. The simultaneous action of TEA leads to the slow release of AI due to properties of TEA - AI complex with 8 = 62.6 ppm. The variation of the results of synthesis for NaA and NaX zeolites may be due to their growth with the participation of different SBU. At the same time, the shape of NaA crystals varies essentially. The contribution of the planes { 110} increases with increase of NHR2 concentration for all systems examined. This dependence is illustrated for NaA crystals grown in the presence of TEA - DEA mixture (Fig. 5). In contrast, the shape of NaX crystals does not change in all cases.
Figure 5. The NaA crystals grown in the presence of TEA- DEA mixture with content of DEA: a-0%; b - 50%; c - 80%; d- 90%; e- 98%; f-100%. Evidently, the synthesis results are strongly influenced by the local chemical composition of the aluminosilicate gel network. They are defined by the proportion and the mutual position of AI and Si in - - O - - S i O---At O - - chains. When a gel is formed, its structure and composition are controlled by the structure and the composition of the initial solutions. Hence the results of zeolite synthesis depend strongly on the structure of AI complexes in the initial solutions. R is well known that Lowenshtein's rule is not violated for zeolite frameworks [2]. Nevertheless, the clear solutions that contain polynuclear complexes of aluminum give the best results for the particle size of NaA and NaX zeolites [9, 10, 13, 14].
156 4. CONCLUSIONS It is shown that amines used as organic additives for NaA and NaX zeolite growths play the role of complex-forming ligands. The structure and the number of alkyl groups in an amine molecule determine the kind of the formed aluminum complex. The changes of the concentration ratio of three different forms of AI complexes influence the zeolite A and X crystal growth. These concentrations depend on the ratio of di- and trialkylamines in the mixture of organic additives. The most important complex for zeolite growth is characterized by the chemical shift 8 = 57 ppm. This complex appears in the presence of DEA or DIPA. Synergism of (NHR2 + NR3) mixture action is observed. The concentration of NHR2 influences the shape of NaA crystals for all systems examined. In contrast, the shape of NaX crystals does not change. ACKNOWLEDGMENTS The authors thank Dr. N. Bogdanchikova for fruitful discussion, and Dr. A. Slavin for careful reading of manuscript. This work was supported by AIST, MITI, Japan. REFERENCES 1. M.E. Davis and R.F. Lobo, Chem. Mater., 4 (1992) 756. 2. D.W. Breck, Zeolite Molecular Sieves, A Wiley Interscience Publ.: New York, 1974. 3. P.A. Jacobs and J.A. Martens, Synthesis of High-Silica Ahminosilicate Zeolites (Stud. Surf. Sci. Cat., Vol. 33), Elsevier: Amsterdam, 1987. 4. S.I. Zones and R.A. Van Nordstrand, in Novel Materials in Heterogeneous Catalysis (Eds. R.T.K. Baker and L.L Murrell) ACS Symp. Set., 437 Am. Chem. Soc.: Washington, DC, 1990, Chap. 2, p. 14. 5. G.O. Brunner, Zeolites, 12 (1992), 428. 6. S.L. Burkett and M.E. Davis, Chem. Mater., 7 (1995) 920. 7. S.L. Burkett and M.E. Davis, Chem. Mater., 7 (1995) 1453. 8. J.F. Charnell, J. Cryst. Growth, 7 (197 l) 29 I. 9. A. Efimov, V. Petranovskii, M. Fedotov, M. Khrepoun and L. Myund, J. Structural Chem., 34 (1993) 548. 10. V.P. Petranovskii, in Proceedings of 9th Zeolite Research meeting, Chem. Soc. of Japan: Tottori, 1993, p. 6. 11. A.W. Apblett, A.C. Warren and A.R. Barron, Chem. Mater., 4 (1992) 167. 12. M. Wiebcke, M. Grube, H. Koller, G. Engelgardt and J. Felshe, Microporous Mater., 2 (1993) 55. 13. V.N. Bogomolov and V.P. Petranovskii, Zeolites, 6 (1986) 418. 14. V.P. Petranovskii, Y. Sugi. Unpublished results. 15. M.G. Voronkov and V.P. Baryshok, J Organomet. Chem., 239 (1982) 199. 16. J.G. Verkade, Ace. Chem. Res., (1993) 483. 17. H. Tayaa, A. Mosset and J. Galy, Europ. J. Solid State Inorg. Chem., 29 (1992) 27. 18. E.N. Coker, P.S. Hees, C.H. Sotak at al., Microporous Mater., 3 (1995) 623. 19. L.V.C. Rees and S. Chandraseckhar, Zeolites, 13 (1993) 528.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
Studies of the Crystallization Gravitational Force Field
157
of ZSM-5
Under High
W. J., Kim1, D. T., Hayhurst2, S. A., Lee1, M. C., Lee1, C. W., LimI and J. C., Yoo1 1Department of Industrial Chemistry, Kon Kuk University, Seoul, Korea 2 D e p ~ e n t of Chemical Engineering, University of South Alabama, Mobile,AL, USA
The 23 factorial method was applied to the crystallization of large ZSM-5 under high gravity to optimize the synthesis condition. The optimum composition was determined and the growth rate, size distribution, and morphology were studied. The activation energies for various systems under high gravity were calculated and found to be consistently lower for elevated gravity synthesis. In addition, the effect of mixing order on the crystallization of ZSM-5 under high gravity was investigated. 1. INTRODUCTION The synthesis of large zeolite crystals has received much attention in both the open and patent literature. Among various zeolites, much attentions have focus~ on the pentasil zeolite, in particular ZSM-5/silicalite. The largest ZSM-5/silicalite are reported to range up to 420 Vm in length[i,2]. Most reports, however, have focused on the optimization of the synthesis mixture. Since the effect of high gravity on the crystallization of silicalite was relx)rted by Hayhurst et al.[3], several investigators[4-8] have reported on high gravity synthesis. According to these reports, high gravity has affects on crystal size, yield and morphology. Although most reports focus on silicalite, there are no report on the preparation of ZSM-5 under high gravity. This is perhaps due to the significant differences in synthesis chemistry between ZSM-5 and silicalite due to aluminum content in ZSM-5. In this research program, the composition of the reaction mixture for synthesis of large ZSM-5 crystal was optimized using 23 factorial method. Experiments were performed at 1 and 30 g. The effects of gravity on the percent crystallization, size distribution and morphology were evaluated.
2. EXPERIMENTAL 2.1. Synthesis The reactants used in this study were a colloidal silica,Ludox AS-40(Du Pont),
158 reagent-grade tetrapropylammonium bromide(Tokyo Chemicals), aluminum nitrate nanohydrate, aluminum hydroxide, 50 wt.% sodium hydroxide solufion(Junsei Chemical Co.) and deionized water. The reaction mixture had the oxide formula, aNa~-bA1203-100SiOz-5TPABr-cI-hO-dGravity where a, b, c, and d were varied by 23 factorial method. The synthesis was designed to perform in four different ways. In scheme I, the reactant solutions were prepared in two beakers. A half of water required , AI(NO3)a.9H20 and 50 wt.% NaOH solution were mixed in beaker I and the remaining water, Ludox AS-40 and TPABr were mixed in beaker If, respectively. After mixing these two solutions separately, they were mixed together and sitrred for enough time to give rise to homogeneous solution. Upon completion of mixing, the reactions were carried out at 180~ under i and 30 g for 24 hours. Scheme II followed exactly the same p r i e s as that of scheme I except that the concentration of Na20 was fixed at 8 moles while the concentration of A1203 was varied from 0.5 moles to 1 mole. In scheme IE based on the 23 factorial experimental results in schemes I and IL 4Na~-100SiO2-3.8TPABr-0.3A12033500H20-xGravity(x = 1 and 30 g) was used as an optimum composition to produce large crystals. The reactions were carried out at 170~ 180~ and 190~ up to 7 days under 1 and 30 g. In scheme IV, the effect of mixing order on crystal growth under high gravity was studied using the same batch composition as an optimized scheme 11I. Unlike schemes I, 1I, and Ill where total NaOH required was added into the alumina solution(be~r I), the amount of NaOH required was divided into two portions by 50%, 70%, and 100%, respectively. It was then added into the alumina solution(beaker I) and the silica solution(beaker II) finally mixing them together. Upon completion of each reaction, linear growth rates were obtained at three different temperatures and the activation energies were calculated. 2.2 Characterization Powder X-ray diffraction analysis(Rigaku Model D/Max-II~) was performed to identify crystallinity and phase. In order to measure crystal size and to investigate morphology, image analyzer(KanImager) and SEM(Shimazu Alpha 25A) were used.
3. RESULTS AND DISCUSSIONS 3.1. Scheme I Following the e ~ m e n t a l procedures described in previous section, the reactions were carried out at 180~ for 24 hours under the same conditions. The compositional ranges for three main factors, namdy, Na~3, H20, and gravity, were varied by 23 factorial method. Thus, each factor was varied from 4 moles, 2 ~ moles, and 1 g, to 8 moles, 3500 moles, and 30 g, res~:tively. Table 1 shows the effect of each combination on crystal size and the combination(bc) has the most significant positive effect while the combination(a) has the most significant negative effect. The negative effect means the decrease in crystal size while the positive effect enhances the crystal size. Aspect ratio(length divided by width) of product crystals was not significantly influenced by gravity.
159 Table 1 Compositional combinations for the effects of different factors on crystal size Crystal size(pm) Effect Significance Combination Factors A B C I II Mean a b ab c ac bc abc
8 4 8 4 8 4 8
2800 3500 3500 2800 2800 3500 3500
1 1 1 30 30 30 30
40.8 50.7 41.1 47.3 24.9 73.6 42.4
43.8 52.3 40.6 44.1 24.1 74.5 39.8
42.3 51.5 40.8 45.7 24.5 74.1 41.1
-20.5 8.9 - 1.3 - 2.2 - 6.5 13.6 - 4.6
+ + -
+ " singinficant at 99 % SEM of ZSM-5 crystals obtained from combinations (a) and (bc) are shown in Figure 1.
a
,~~
Ilc
,..~2
Figure. 1. SEM of ZSM-5 obtained from combinations (a) and (bc) Conversely, the crystallinity decreased slightly with high levels of I-~O and gravity. In order to identify the phase of solid product and crystallinity, x-ray powder diffraction analysis was performed and the crystallinity for each combination was calculated by the area between 22.5~ and 25~ in 29. Figure 2 shows XRD pattern of product obtained from combination (b) and no other phase except ZSM-5 was found. The crystallinity for each combination was summarized in table 2. Increasing the concentrations of I-IzO and gravity resulted in a slight decrease in crystallinity due to the majority of nucleation and crystallization occuring at the interface between the top-liquid phase and the segregated solid gel. As a conclusion, the gravity does not have significant effects on crystallinity while it enhances the crystal size significantly. Furthermore, it is interesting that the effect of gravity on the size distribution strongly depends on the concentration of I-hO as shown in Figure 3. At the low concentration of I-I20, the gravity resulted in positive effects on size distribution(narrow size distribution) while the gravity showed a negative effect on size distribution at the high concentration of I-I20.
160
GO 13.. 0
5.00 10.00
20.00
20
30.00
40.00
5000
Figure 2. XRD pattern of product obtained from combination (b) Table 2 Compositional combinations for the effects of different factors on crystallinity Effect Significance Combination Factors Crystallinity A B C I II Mean a b ab c ac bc abc
8 4 8 4 8 4 8
2800 3500 3500 2800 2800 3500 3500
1 1 1 30 30 30 30
96.9 98.9 98.2 96.5 98.4 96.4 72.8
96.9 96.9 97.7 100.0 97.7 96.4 82.8
96.9 97.9 98.0 98.3 98.1 96.4 82.8
-
4.6 5.0 4.6 4.7 4.8 6.1 4.6
+ -
+ " significant at 99 % 3.2. Scheme II In scheme II, AlzOa, I-hO and gravity were the parameters that were varied from 0.5 moles, 2800 moles and 1 g to 1.0 mole, 3500 moles and 30 g, respectively. In this case, the concentration of Na20 was fixed at 8 moles and the reaction was carried out for 1 day. As shown in table 3, an interesting result is that the crystal size was increased with aluminum content under high gravity while vice versa under 1 g. The effect of gravity on the crystal size seemed to become significant as aluminum content increased; that is, regardless of I-hO content, the crystal size decreased by 6 to 38% upon increasing aluminum content at 1 g while it was significantly enhanced at 30 g by 17% to 47%. This is attributed to the greater consumption of aluminum for crystal growth rather than for nucleation due to the liquid-solid segregation resulting from applying gravity. In case of crystallinity, combination(bc) in which I-hO content and gravity were high shows a negative effect on crystallinity indicating that gravity is not important as shown in table 4.
161 (a)
25
I
w
~,20
I
i
.:""~-->30G
o 10
....m.,':
7=0
(b)
/
/~\-I
"'" . ".. / /
35 _ ,
,
30
~'25 "6 20 '- 15 E 10
0
--1
=
Z
1 .i i t 40 50 60 Crystal Size(um)
5
0
! --
~
1G<--! .
_,'
i.
i .__2-.~ 1 20 30 40 Crystal Size(um)
50
(d)
(c) m
,4--= r
4O 35
~, 30 0 25 o 20 .Q r 115 -
\-->IG
0 5 0
_
\
_
E z
3O 1 25 0 20 -o 15 -Q 10 E = 5 j~ z 0 30
I 1).._~,
m
I
I - - - I .
_
I..
3OG<-:.
-
L
50
.,/ /
NI--
9
';
.
: -
60 70 80 Crystal Size(um)
9
I
I
-
l-->lG I
--
'~
I H
,,-
t
-
40 50 60 Crystal Size(urn)
Figure 3. Comparisons of the size distributions for the samples obtained from xNa20-0.5AI~O3-100SiO2-5TPABr-yH20 under 1 and 30g, respectively" (a) x=4, y=2800, (b) x=8, y=2800, (c) x=4, y=3500, and (d) x=8, y=3500. Table 3 Compositional combinations for the effects of different factors on crystal size Effect Significance Crystal size(pm) Combination Factors A B C I II Mean a b ab c ac bc abc +
1.0 0.5 1.0 0.5 1.0 0.5 1.0
2800 1 3500 1 3500 1 2800 30 2800 30 3500 30 3500 30
28.1 41.1 38.8 24.9 34.7 42.4
47.1
24.6 40.6 37.5 24.5 38.0 39.8 48.9
26.4 40.9 38.2 24.7 36.4 41.1 48.0
- 0.03 9.6 2.1 0.6 9.3
m
+ +
4.4
-
4.5
-
9significant at 97.5%
3.3. Scheme I n Based on the results obtained from schemes I and IL the optimum composition for large crystal was determined. It was for NaOH and alumina as low as possible and for I-hO and gravity as high as possible. The molar composition was
162 Table 4 Compositional combinations for the effects of different factors on crystallinity Combination Factors Crystallinity Effect Significance A B C I II Mean a b ab c ac bc abc
1.0 0.5 1.0 0.5 1.0 0.5 1.0
2800 1 3500 1 3500 1 2800 30 2800 30 3500 30 3500 30
84.0 98.2 100.0 98.4 89.9 72.8 90.4
87.3 97.7 81.5 97.7 94.8 82.8 79.4
85.7 97.9 90.8 98.1 92.4 77.8 84.9
- 4.3 - 5.4 4.2 -4.5 5.0 -8.5 2.2
+ " significant at 97.5 % 4Na20-100SiO2-3.8TPABr-0.3AI2(h-~H20. The reactions were carried out at three different temperatures up to 7 days. Figures 4 (a) and (b) show the aveyage crystal size with reaction time at 1 and 30 g.
(a) 1 G
v
(b) 3 0 G
E
E -!
v
w U oO
w
oo
~< .J
.J
Q: O
rr (3
0
1
2
3
4
5
REACTION TIME(HRS)
6
7
0
1
2
3
4
5
6
7
REACTION TIME(HRS)
Figure 4. Average crystal size vs. reaction times for the crystal obtained at various temperatures under (a) 1 g and (b) 30 g. The average crystal size with time at 190~ was significantly fluctuated in case of 1 g while the average crystal sizes with time were increased in proportion to temperature for 30 g. It also can be realized that the size distribution of crystals obtained at individual time interval for 30g was much narrower than that for 1 g. In addition, the maximum crystal sizes at each individual time for 170~ 180~ and 190~ were shown in Figures 5 (a) and (b) to investigate the reaction kinetics for crystal growth under 1 and 30 g. As shown in these Figures, the crystal sizes of ZSM-5 for three different temperatures show linear growth rotes up to 24 hours. The activation energies were calculated from the crystallization curve slope where a linear growth rate is observed. The activation energies of 63.19 kJ/mol and 56.54
163 (b) 30 G
(a) 1 G 160
19o"c
9
o-180='c
E
160
~ 120-
O''''C
.._.1
~ 80
~80.
D 40
~ 40.
>-. nO
Z~:lgO~ O:180~ O:170~
X
< ~
0
0
4
8
12
16 20 24
REACTION TIME(HRS)
0
4
8
12 16 20 24
REACTION TIME(HRS)
Figure 5. Maximum crystal size vs. reaction time for the crystal obtained at various t e ~ a t u r e s under (a) 1 g and (b) 30 g. kJ/mol were obtained for 1 g and 30 g, respectively. Lower activation energy for 30 g might be attributed to the fast crystal growth due to tl~ limited crystallization mainly at liquid-solid interphase. The value, 63.19 kJ/mol for 1 g is fairly consistent with 64.5 kJ/mol reported by Feokfistova et all9]. 3.4. S c h e m e IV
In scheme IV, the effect of mixing procedure in preparing reactant solution on crystal growth rate was studied using the same molar composition as that of scheme HI.. Unlike schemes I, ]l, and Ill where total NaOH solution required added into alumina s o l u f i o n ( ~ e r I), the reactant solutions were prepared in three different ways ; those are, 50%, 70% and 100% of 50 wt.% NaOH solution required were added into the silica solution(beaker II), respectively. The reactions were carried out at 170~ 180~ and 190~ under 1 and 30 g up to 24 hours. The logarithmic plots of the linear rate of ZSM-5 crystallization with respect to reciprocal temperature for 1 and 30 g were shown in Figures 6 (a), (b) and (c). In case of adding a half of 50 wt.% NaOH solution into silica containing solution, the activation energies for 1 and 30 g are 68.17kJ/mol and 64.85 kJ/mol(Fig.6(a)). However, as the addition of 50 wt.% NaOH solution into silica solution increased to 70% of total NaOH required(Fig.6(b)), the difference in the activation energies for 1 and 30 g became larger than that of the previous case. The activation energies for 1 and 30 g are 61.52 kJ/mol and 51.55 kJ/mol, respectively. This might be attributed to the more dissolution of highly stable silica particles upon addition of NaOH solution. On the other hand, the activation energies for the case of adding total NaOH solution required into the silica solufion(Fig.6(c)) increased to 66.51 kJ/mol and 59.85 kJ/mol for both 1 and 30 g compared to the second case. This seems to be caused by the formation of much more silicate species which could require more activation energies. It is interesting, however, to note that the activation energy under high gravity is smaller than under normal gravity regardless of mixing procedures.
164 (a)
(b)
(c) 1.85
1.85
1,85
,,r
~= 1.35
_=1.35
-%.,o .
lIT X IO00(K)
%
2~
lIT X IO00(K)
2ao
0 ~
I-
2.10
:
.~
.
220 230 1/T x IO00(K)
Figure 6. Logarithmic plots of the linear rate of ZSM-5 crystallization vs. reciprocal temperature for 1G and 30G.
4. CONCLUSIONS Several conclusions were obtained through this work. The gravity does not have significant effects on % crystallization while it enhances the crystal size significantly. In addition, the results suggest that the effect of gravity on the size distribution strongly delxmds on the concentration of I-hO. At low concentration of H ~ , the gravity resulted in narrow size distribution while it caused broad size distribution at the high concentration of I-hO. Unlike normal gravity, aluminium content shows positive effects on crystal size under high gravity. Finally, regardless of mixing procedures, a high gravity gives rise to lower activation energy than a normal gravity.
REFERENCES
1. D.T. Hayhurst and J.C. Lee, in New Developments in Zeolite Science and Technology(Fxts. y. murakami, A. Iijima and J.W. Ward) Kodansha, Tokyo and Elsevier, Amsterdam(1986),239. 2. J. Komatowsld, J. Zeolites 8(1988), 77. 3. D.T. Hayhurst, P. J. Melling, W. J. Kim and W. bibby, Zeolite Synthesis, ACS Symp. Set. No. 398(Eds. M..L. Occelli and H.E. Robson)(1989), 233. 4. W.J. Kim, Ph.D. Dissertation, Cleveland State University(1989). 5. W.J. Kim and J. Lee, J. Korean Ind. & Eng. Chem. Vol. 2, No. 2(1991), 97. 6. H. Zhang, S. Ostrach and Y. Kamotani, Trans~rt Phenomena in Materials Processing and Manufacturing, HTD-Vol. 196(1992). 7. H. Zhang, S. Ostrach and Y. Kamotani, 31st Aerospace Sciences Meeting and Exihibit, 1(1993), 11. 8. H. Zhang, S. Ostrach and Y. Kamotani, Processings of 10th International Conference on Crystal Growth(1993). 9. N.N. Feoktistova and S.P. Zhdanov, Zeolites Vol. 9(1989), 5.
H. Chon, S.-K. Ibm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
165
Structure directing role o f N a + and T M A + cations in 18-crown-6 ether mediated crystallization o f EMT, M A Z and SOD aluminosilicate zeolites E.J.P. Feijen, B. Matthijs, P.J. Grobet, J.A. Martens and P.A. Jacobs Centrum voor Oppervlaktechemie en Katalyse, KU Leuven Kardinaal Mercierlaan 92, B-3001 Heverlee (Leuven), Belgium
Summary
Zeolite crystallizations are performed in the system 10 SiO2; 1 A1203; 0.97 18-crown-6 ether; x Na20; y TMA20; 135 H20. EMT, MAZ and SOD type phases are obtained depending on the relative concentrations of sodium and TMA in the gel. The nature of the phases obtained is rationalized by the extended-structure approach with specific structure directing roles for the different cations in the formation of extended structures as well as in their mutual condensation.
1. INTRODUCTION Although much progress has already been made in the identification of precursors and template effects, the crystallization mechanisms responsible for the formation of zeolites are not yet fully understood [1]. According to the extended-structure approach of zeolite crystallization, zeolites grow by condensation of extended-structures (ES) whereby primary cations template the formation of ES units, and secondary cations organize the condensation of ES units [2]. Recently, this approach has been validated in the crystallization of FAU and EMT phases and their intergrowths in the presence of crown-ethers [3]. A mechanism of condensation of faujasite sheets decorated with the crown-ether molecules rationalizes and quantitatively predicts the exact nature of the faujasite polytype with respect to intergrowth pattern and phase composition. In this work, a hydrogel leading typically to the crystallization of the EMT phase was modified by adding tetramethylammonium cations (TMA) and varying the concentration of sodium. From these systems, EMT, MAZ and SOD zeolite phases were obtained. The nature of the zeolite phases obtained can be rationalized based on the known primary and secondary structure directing roles of sodium, TMA and sodium-crown-ether complexes. 2. EXPERIMENTAL Hydrogels were prepared with the following standard molar composition: 10 SiO2; 1 A1203; 0.97 18-crown-6 ether; x Na20; y TMA20; 135 H20. The Na and TMA contents of the gel are summarized in table 1. The 18-crown-6 ether (1,4,7,10,13,16-hexaoxacyclooctadecane, Janssen Chimica) was added to a colloidal silica source (Ludox HS-40). Gibsite (Fluka) was dissolved in an aqueous solution of NaOH and TMAOH under heating at 353K. The latter solution and the silica sol were combined and stirred for 15 minutes. The gels were transferred
166 into teflon lined autoclaves and aged at room temperature for 3 days. Crystallization was interrupted after 9 days of heating at 373K. The solids were recovered by centrifugation at 39 kG and washed with deionized water until the pH of the wash water was lower than 9. X-ray diffraction patterns were recorded on an automated Siemens D5000 diffractometer. Infrared spectra were taken on a Nicolet 730 FTIR spectrometer using the KBr pellet technique. Scanning electron micrographs on gold-coated samples were obtained using a Jeol superprobe 733 instrument. Thermogravimetric analyses and differential thermoanalysis profiles were recorded on a Setaram TGA 92 thermobalance in oxygen/helium (20/80 vol/vol) atmosphere. 13C MAS NMR with proton decoupling was performed on a Bruker 400 MSL spectrometer at 100.6 Mhz., with a pulse length of 4gs, a repetition time of 10s and a spinning rate of 4kHz. Quantitative 27A1 MAS NMR spectra were recorded on the same spectrometer at 104.2 Mhz, with a pulse length of 0.61 gs, a repitition time of 0.1 s and a spinning rate of 14 kHz using zeolite samples with the same topology and known A1 content as references.
3. RESULTS AND DISCUSSION 3.1. Gel composition and crystallization products The crystalline phases present in the products, as determined by XRD, are summarized in Table 1. In a first series of experiments (series A: sample 1 to 5), the influence of the addition of TMA cations to the gel was studied. The experiment in absence of TMA (sample 1), is a typical 18-crown-6 ether mediated crystallization of the hexagonal faujasite phase (EMT). Gradual addition of TMA cations yields the co-crystallization of more MAZ phase next to traces of SOD. XRD studies of series A showed, however, that the crystallization of MAZ which is most abundant in sample 2, (Figure 1) is suppressed at increasing TMA levels, the SOD phase becoming more abundant (sample 5, Figure 2). The weakly intense diffraction lines at a 2e value of 6 ~ in sample 2 indicate the presence of traces of EMT (Figure 1). The SEM picture in Figure 5 shows that the MAZ phase in sample 2 consists of spherulitic crystals, with a diameter of 1 to 2 gin. The spherulitic morphology is typical of MAZ type zeolite crystals grown under conditions of high supersaturation [4].
Table 1 Na20 (x) and TMA20 (y) concentrations in the standard hydrogel and XRD-visible crystalline phases I
Sample
x
y
Phases in product
Sample x
y
Phases in product
2.04
0.48
MAZ>EMT, SOD
8
1.92
0.48
MAZ>EMT
9
2.30
0.24
MAZ>EMT, SOD
2.21
0.24
MAZ > EMT, SOD
11
2.16
0.24
MAZ> EMT
MAZ>EMT, SOD Ij 12
1.68
0.72
SOD
!
1
2.40
0.00
EMT
i7 I
2
2.40
0.24
MAZ>EMT, SOD
3
2.40
0.48
MAZ>EMT, SOD I
4
2.40
0.72
MAZ>EMT, SOD . 10 I
5
2.40
0.96
SOD>MAZ I
6
2.28
0.48
167
I
5
l
I
l0
l
I
,
I
I
.
t
15 20 25 30 35 40 45 50 55 2O
Figure 1: XRD pattem of sample 2.
1'o1'5 ' ~o' ~5' ~o' ~5' ~o' ~5' go 55 2O Figure 2: XRD pattern of sample 5.
1 5
10 15 20 25 30 35 40 45 50 55 20 Figure 3: XRD pattem of sample 10.
' lb' l'5' J.o ~
~o ~5 do ,is go' 55 2O
Figure 4: XRD pattern of sample 12.
In order to further examine the influence of sodium and TMA cations, additional series of experiments were set up with variable amounts of sodium at a constant TMA content (series B: sample 6 to 8; series C: sample 9 to 11). For series B, all samples contain a considerable amount of MAZ and SOD, and possibly traces of EMT. In series C, three phases (EMT, MAZ and SOD) were unambiguously identified as illustrated with the XRD pattern of sample 10 (Figure 3). The SEM picture of sample 11 in Figure 6 clearly shows physical mixtures of hexagonal crystals of the EMT phase and spherulitic crystals assigned to the MAZ phase. Abundant TMA addition results eventually in the crystallization of the dense SOD phase only (sample 12, Figure 4). The Si/A1 ratio of the SOD phase of sample 12 is 6.3 according to quantitative 27A1 MAS NMR. For these experiments it is concluded that from Na and 18-crown-6 ether containing hydrogels, the crystallization of EMT is readily suppressed by addition of TMA. Instead, the MAZ phase is preferred at intermediate TMA contents in the hydrogel, while from TMA-rich hydrogels, a pure SOD phase crystallizes under the conditions investigated.
168
Figure 5: SEM picture of sample 2.
Figure 6: SEM picture of sample 11 (after 6 days of heating).
3.2. Quantification of phases in zeolite mixtures
During zeolite crystal growth, TMA cations are often occluded in cavities such as gmelinite and sodalite cages. Such occlusion phenomena of TMA have been observed previously for the crystallization of mazzite and sodalite type zeolites [5,6]. Thermoanalysis profiles confirm the presence of TMA cations in the present samples (Figures 7 and 8). The oxidative decomposition of TMA in gmelinite and sodalite cages is observed at 820 and 870 K, respectively. From the TG profile in Figure 8, the TMA content of sample 12 containing only SOD could be estimated. It was found that approximately each sodalite cage contains 1 TMA. The presence of these cations in gmelinite and sodalite cages was confirmed by Hdecoupled 13C MAS NMR. Indeed, for sample 2, the spectrum in Figure 9 shows resonance lines at 58.8 and 57.9 ppm, indicating the presence of sodalite cage and gmelinite cage occluded TMA cations, respectively [7]. Furthermore, a weak resonance is observed at 70 ppm, originating from Na-18-crown-6 ether complexes in the EMT structure [3,8]. These findings are in good agreement with the presence of three phases, viz. MAZ, SOD and EMT according to the XRD analyses (Table 1 and Figure 1). The amount of MAZ and SOD derived from the amount of TMA decomposed at 820 and 870 K, respectively, is plotted in Figure 11 against the Na20/(Na20 + TMA20) ratio in the synthesis gel. The amount of EMT in the samples (Figure 11) was estimated based on the intensity of the Double 6 Ring (D6R) vibration in the IR spectra, relative to that of the TObending vibration (450 cm 1) [3]. For sample 11, the IR spectrum is displayed in Figure 10.
169 The D6R vibration (585 cm l ) is clearly present as a shoulder at lower frequency on the Single 6 Ring vibration band (621 cm 1) of the MAZ structure.
3.3. Crystallization mechanism It is evident from Figure 11 that there is a relationship between the fraction of the Na/(Na+TMA) cations in the synthesis mixture and the formation of a particular structure type. Indeed, only intermediate fractions yield MAZ type zeolites, while from Na-rich and TMA-rich gels preferentially the EMT and SOD type zeolites are crystallized, respectively.
75
0
0
TG
150 50
-5
100~
~ ~ -lO
-10
-15 t t a Flow
0
'
~
'
460
'
660
'
-20
'
200
'
Terrp (~
Ternp (~
Figure 8:TG-DT analysis profile of sample 12.
Figure 7" TG-DT analysis profile of sample 11.
0.6
0.5
i~ 0.3
32' ~0' gS' 6'6 ' 6'4 ' g2 ' 6'0 ' 5'8 ' 5P6 (ppm)
O.
1000
~ Wa~nt~
Figure 9" 13C MAS NMR profile of sample 2
1~
~
~
5(~0 ' 4t~
(crab
Figure 10: IR spectrum of sample 11.
170
9
9 9
80 o~
~,,,,,,
9
40
20
.
",,,,.
/ .
mA
0.75
0.-80
- 0.85
0.-9ff
0.95
1
Na20 / Na20 + TM~O Figure 11" Influence of the Na and TMA content of the synthesis mixture on the crystallization of EMT, MAZ and SOD.
Following the extended-structure approach [2,3], the Na and TMA cations are classified as primary cations, responsible for the formation of extended structures (ES) during crystallization. For the formation of EMT and MAZ phases, these ES units are faujasite and mazzite sheets, respectively (Figure 12). The secondary cations that control ES condensation are Na-crown-ether complexes [3] and Na ions (Figure 12), respectively. Indeed, only Na and TMA cations were found in the MAZ materials, the latter cations being exclusively present in the gmelinite cages being part of the ES units. The crystallization pathways drawn in Figure 12, with each pathway controlled by specific primary and secondary cations, now fully explain the formation of the different zeolite types (Figure 11). Indeed, in absence of TMA, only pathway A is available, and EMT formation dominates. In presence of Na and TMA, pathway B becomes possible as mazzite sheets can be formed. Indeed, Na acts as primary as well as secondary cation for MAZ, and is assisted by TMA and its templating effect for gmelinite cages. If TMA cations become more abundant compared to Na, the structure directing potential of TMA for sodalite cages leads to SOD phases built from condensed sodalite cages. For reasons of charge compensation in the lattice, these TMA containing sodalite cages cannot be organized into an 18-crown-6 ether containing EMT lattice [3]. Pathway B, yielding MAZ, also becomes unfavourable under these conditions, as the concentration of sodium, i.e. a primary as well as secondary cation, is too low.
171
SOD
mazzite sheet
fauj asite sheet
+
i.
TMA Na+ _. TMA+
Na+1
( ~
Na+
[ [Na-18-crown-6]
g/
MAZ
EMT
Figure 12: Crystallization routes for EMT, MAZ and SOD.
4. CONCLUSIONS The crystallization of EMT, MAZ and SOD type aluminosilicate zeolites is controlled by the relative amounts of Na and TMA in the synthesis hydrogel. Their effect on the nature of the crystalline products is explained by their specific structure directing contribution in the formation of extended structures and the further organization of these units into a crystalline zeolite lattice.
ACKNOWLEDGEMENTS
This work is sponsored by the Belgian Ministry of Science Policy in the frame of an IUAP-PAI program and by the Flemish N.F.W.O. EJPF acknowledges KU Leuven for a postdoctoral fellowship, JAM and PJG the Flemish NFWO for a research position.
REFERENCES
1 E.J.P. Feijen, J.A. Martens and P.A. Jacobs, Zeolites and Related Microporous Materials: State of the Art 1994 (part A), Studies in Surface Science and Catalysis, Vol. 84., J.
172
2 3 4
5 6 7 8
Weitkamp, H.G. Karge, H. Pfeifer and W. H/51derich (Editors), Elsevier Science B.V., Amsterdam, (1994) p.3. D.E.W. Vaughan, Catalysis and Adsorption by Zeolites, G. Ohlmann, H. Pfeifer and R. Fricke (Editors) Elsevier Science B.V., Amsterdam (1991) p.275. E.J.P. Feijen, K. De Vadder, M.H. Bosschaerts, J.L. Lievens, J.A. Martens, P.J. Grobet and P.A. Jacobs, J. Am. Chem. Soc., 116 (1994) 2950. F. Di Renzo, F. Fajula, F. Figueras, S. Nicolas and T. Des Courieres, Zeolites" Facts, Figures, Future, Studies in Surface Science and Catalysis, Vol. 49 A., P.A. Jacobs and R.A. van Santen (Editors), Elsevier Science B.V., Amsterdam, (1989) p. 119. R.M. Barrer, Hydrothermal Chemistry of Zeolites, Academic Press, London (1982) p. 166. C. Baerlocher and W.M. Meier, Helv. Chim. Acta., 52 (1969) 1853. S. Hayashi, K. Suzuki, S. Shin, K. Hayamuzi and O. Yamamoto, Chem. Phys. Let. (1985) 368. F. Delprato, L. Delmotte, J.L. Guth and L. Huve, Zeolites 10 (1990) 546.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 i997 Elsevier Science B.V. All rights reserved.
173
Synthesis of high-silica FAU-, EMT-, RHO- and KFI-type zeolites in the presence of 18-crown-6 ether. T. Chatelaina, J. Patarina, E. Brendl~a, F. Dougniera, J.L. Gutha and P. Schulzb a Laboratoire de Mat~riaux MinOraux URA-CNRS 428 ENSCMu - UHA 3 rue Alfred Werner, 68093 Mulhouse Cedex, France b Centre de Recherche Elf Antar-France de Solaize, Chemin du Canal, BP22, 69360 Saint Symphorien d'Ozon, France FAU-, EMT-, RHO- and KFI-type zeolites were synthesized by heating an aqueous alkaline aluminosilicate gel containing 18-crown-6 ether as an organic template with either sodium, or sodium and cesium, or potassium and strontium cations. The products were characterized by elemental analysis, scanning electron microscopy , powder X-ray diffraction , thermal analysis, solid-state nuclear magnetic resonance spectroscopy, and n-hexane adsorption. The 18-crown-6 ether is incorporated in each structure. Its presence turns out to be necessary to crystallize EMT-type materials and, in the other cases, it allows reproducible preparations of well crystallized materials with high Si/AI ratios (3.7-4.6). The retrieval of the 18-crown-6 ether from the EMT-type zeolite is possible with solvothermal treatments. Keywords
Synthesis, high-silica zeolites, 18-crown-6 ether
1. INTRODUCTION
Recently, in our laboratory the use of crown-ethers in an aluminosilicate gel containing sodium cations led to the crystallization of high-silica FAU- and EMT- type zeolites [1]. Later, other studies have been published on these materials [2-4]. Knowing the industrial interest for these high-silica zeolites [5], an extensive optimization work has been performed in order to decrease their synthesis cost. Moreover, as other zeolites have pores which are potentially able to accomodate crown-ether-cation complexes, a synthesis study was undertaken with different alkaline cations associated with 18-crown-6 ether. The aim was to increase the Si/AI ratio of zeolites already known and to take advantage of the structure-directing effect of crown-ether for developing more specific synthesis procedures for these zeolites. 2. EXPERIMENTAL 2.1. Reactants
The reactants were 18-C-6 ether (1,4,7,10,13,16-hexaoxacyclo-octadecane, > 98%, Lancaster), sodium hydroxide (purum, > 98%, Fluka), potassium hydroxide (normapur, > 86%, Prolabo), cesium hydroxide (50wt% CsOH, 50wt% H20, Aldrich) and strontium nitrate (normapur, >99%, Prolabo). The silicon and aluminum sources
174
were colloidal silica (40wt% SiO2 in water, CecasoI,Ceca or Ludox AS40, Du Pont de Nemours ) and sodium aluminate (56wt% AI203, 37wt% Na20, Carlo Erba) or aluminum hydroxide (purum, 65 wt% AI203, Fluka).
2.2. Synthesis procedure for the FAU-, EMT- and RHO-type materials
The samples were obtained by hydrothermal synthesis at 110 ~ optimization, the molar composition of the starting mixtures was as follows:
After
10 SiO2 : 1 AI203 : x Na20 :y Cs20:0.4-0.5 (18-crown-6) : 100 H20 where x = 2.6 and y = 0 for FAU-type zeolite; x = 2.1 and y = 0 for EMT-type zeolite; x = 1.1-1.8 and y = 0.3 for RHO-type zeolite. In all three cases, the starting mixture was prepared according to method II described elsewhere [6,7]. The resulting gel was aged at room temperature for 24 hours in a closed polypropylene bottle under continuous stirring. The crystallization was carried out under static conditions in PTFE-lined stainless-steel autoclaves during 2 to 15 days. The solids obtained were filtered, washed with distilled water until the pH of the filtrate was neutral and then dried at 80 ~
2.3. Synthesis procedure for the KFI-type materials
The samples were obtained by hydrothermal synthesis at 150~ composition of the starting mixture was:
The molar
10 SiO2 : 1 AI203 : 1.8-2.3 K20:0.10 SrO :0.5-1.0 (18-crown-6) : 160-220 H20 The synthesis procedure was similar to that developed by Verduijn [8]. A mixture of KOH and AI(OH)3 with a portion of water was boiled, under continuous stirring, until a clear solution A was formed and then cooled to room temperature. Sr(NO3)2 and 18-crown-6 were successively dissolved in another portion of water and colloidal silica was slowly poured in the thoroughly stirred solution before adding solution A. Before heating under static conditions in PTFE-lined stainless-steel autoclaves during 4 to 5 days, the resulting gel was stirred for about 30 minutes. After crystallization, the products were treated as previously described. A classical KFItype zeolite sample, i.e., without organic species, was also prepared according to the procedure described by Verduijn [8].
2.4. Chemical analysis
Si, AI, Na, K, Cs and Sr analysis was performed by atomic absorption spectroscopy. The amount of water and organic species of the as-synthesized materials was determined by thermogravimetry. Carbon analysis was performed by coulometric determination after calcination of the samples at 1050 ~ under air.
2.5. Powder X-ray diffraction
The powder patterns were obtained on a Philips PW 1800 diffractometer equipped with a variable divergence slit (CuKo0. For the FAU-type materials the relative XRD intensity was determined according to the ASTM D3906-85a procedure [9]. A similar procedure was set up for the EMT samples (18 peaks in the 2e range 1530~ and for the RHO-[7] and KFI-type materials.
2.6. Thermal analysis
Prior to analysis, the solids were equilibrated over a saturated aqueous solution
175
of NH4CI (p/po=0.85). Thermogravimetry (TG) was performed on a Mettler 1 thermoanalyzer by heating in air at 4~ -1. Differential thermal analysis (DTA) was carried out in air on a BDL-Setaram M2 apparatus between 20 and 750 ~ at a heating rate of 10 ~
2.7. Adsorption measurements The sorption studies were carried out on protonated samples, obtained according to a procedure previously described for FAU and EMT zeolites [10]. The adsorption capacity measurements were performed by using a computerized thermogravimetric equipment TG 92 from Setaram. About 100 mg of the calcined solid was activated at 450~ under flowing dry N2 (heating rate : 5~ After 1 hour at 450 ~ the sample was cooled to room temperature during 1 hour. Then the solid was subjected to a flowing mixture of dry nitrogen and n-hexane, during 10 hours. The relative pressure P/PO of n-hexane was 0.5. 2.8. 13 C,27AI, 29Si solid-state MAS and CP MAS NMR spectroscopy The spectra were recorded on a Bruker MSL 300 spectrometer. The recording conditions of the CP MAS and MAS spectra are given in ref.7. 2.9. Determination of the occluded organic species by liquid 1H NMR A known amount of the as-synthesized zeolites (~ 80 mg) was dissolved into 1.5 cm3 of a 40 wt% aqueous HF solution. Thereafter 200 mg of a lwt % dioxane-D20 solution was added as internal standard to the dissolved zeolites. After centrifugation, ,,, 0.5 cm 3 of the liquid was transferred with an equivalent volume of pure D20 in a PTFE tube. The latter was then placed in a classical glass tube for the NMR analysis. The spectra were recorded on a Bruker AC spectrometer. The recording conditions were: frequency =250.13 MHz; recycle time =8 s; pulse width =2 ms; pulse angle = 30 ~ 2.10. Retrieval of 18-crown-6 ether from EMT zeolites The retrieval of the 18-crown-6 ether was performed by a solvothermal treatment of a suspension of the as-synthesized zeolitic samples in water or in an alcohol with or without a salt at a temperature ranging from 180~ to 200~ 3.RESULTS AND DISCUSSION 3.1.Synthesis, crystal morphology, chemical composition and thermal analysis In the absence of Cs + cations and for x= 2.1, a pure EMT zeolite could be synthesized with a lower amount of the expensive 18C6 ether. Indeed, the previously used stoichiometry was reduced from 0.7 [1-4] to 0.4 (Table 1, sample D). Under these new synthesis conditions, no 18C6 remains in the mother liquor. A scale-up study has shown that with this new gel composition, batches producing several kilograms of very pure EMT-type zeolite were easy to reproduce [11].For x = 2.6, the soda content is too high for the 18C6 ether to direct the crystallization towards the EMT structure-type, the FAU phase was obtained (see Table 1, sample A ). For intermediate values ( 2.1<x< 2.6), intergrowths or overgrowths (FAU/EMT) of the two structural types were produced (Table 1, sample C). For instance, according to Treacy et al.[12], an (x value close to 0.5 was found for x= 2.4. In the absence of 18C6 ether, the materials were amorphous(see sample B) and no EMTtype zeolite could be obtained.
176
Table 1 Typical synthesis conditions of FAU-, EMT-, or RHO-type zeolites (starting molar gel composition : 10 SiO2 : 1 AI203 : x Na20: y Cs20 : z18-crown-6 : 100 H20). Heating time Sample x y z at 110~ XRD results (estimated crystallinity) a (days) A 2.6 0.0 0.4 8 FAU (100%) B 2.6 0.0 0.0 8 Amorphous C 2.4 0.0 0.4 8 FAU/EMT (or,~ 0.5) D 2.1 0.0 0.4 8 EMT (100%) E 1.8 0.3 0.5 8 RHO (100%) F 1.8 0.3 0.5 2 RHO (90%) G 1.8 0.3 0.0 2 RHO (45%) + CHA b + ANA b + amb H 1.1 0.3 0.5 15 RHO (90%) a : The reference samples are A for FAU materials and E for RHO materials. b : CHA = chabazite, ANA = analcime, am : amorphous material. The partial substitution of cesium for sodium in the gel composition (1.1< x< 1.8) gave rise to the crystallization of a pure high-silica RHO -type zeolite [7]. Here also the use of crown-ether seems to be necessary for obtaining a pure phase with good reproducibility. As a matter of fact, without the crown-ether molecule in the starting mixture, only a poorly crystalline RHO material was obtained with some chabazite and pollucite [( Na, Cs) analcime] as by-products (compare samples F and G). As it has been observed above for the RHO-type solids, the introduction of 18-C6 in the starting mixture of a KFI-type zeolite led also to a pure material (compare samples I and M, Table 2). Whereas, in the case of RHO zeolite, the soda content can be decreased to x=1.1, the K20 amount (k) has to be close to 2.3- 2.5 otherwise no crystallisation occurs after 5 days (see Table 2, sample L). Table 2 Typical synthesis conditions of KFI-type zeolites. Starting molar gel composition : 10 SiO2 : 1 AI203 : k K20:0.10 SrO :t 18-crown-6 : w H20 Heating time Sample k t w at 150~ XRD results (estimated crystallinity) a (days) Ib 2.3 0 160 5 KFI (90%) + (n.i.)c J 2.3 1 220 5 KFI (100%) K 2.3 0.5 160 5 KFI (90%) L 1.8 1 160 5 Amorphous M 2.3 1 160 5 KFI (100%) a : The reference sample is sample M b : Sample prepared according to the procedure described in ref. 8 c : (n.i.) Traces of a unidentified impurity The FAU-type crystals display a typical octahedral morphology (Figure l a), whereas the EMT-type samples consist of fairly hexagonal platelets (Figure lb). In the latter case, a decrease of the 18-crown-6 ether content (0.4 instead of 0.7) [1-4] and of the water content (100 H20 instead of 140 H20) [1-4] led to a significant
177
decrease of the crystal size (1-21~m instead of 3-4pm) which should enhance the activity of this zeolite in catalytic craking reactions. The RHO-type samples prepared in the presence of crown-ether display a sphere-like shape with an average size of ll~m (Figure lc). Whereas, aggregates of cubic crystals with a size close to 3-41~m were obtained for the KFI-type materials (Figure 1d).
(b)
(c)
(d)
Figure 1. Scanning electron micrographs of high-silica zeolites: (a) FAU sample A; (b) EMT sample D; (c) RHO sample E; (d) KFI sample M The chemical composition of some samples is reported in Table 3. The framework Si/AI molar ratios determined by 29Si MAS NMR spectroscopy are in good agreement with the values obtained from chemical analysis. This confirms that there is no extra-framework aluminum species in the as-made samples as checked by 27AI NMR spectroscopy and that no unreacted gel is present. Zeolites, whose synthesis is possible without crown-ether, i.e., FAU-, RHO- and KFI-type zeolites, show higher Si/AI ratios when the synthesis is performed in the presence of 18C6 ether. There are probably three reasons for this: -for a given Si/AI ratio in the gel, crystallization is generally possible with a lower alkalinity which does not favor the AI incorporation. -the incorporation degree of the bulky 18C6-cation complex is lower and consequently the substitution of AI for Si. -the 18C6-cation complex has better stabilization interactions than hydrated cations when the hydrophobicity of the framework increases (higher Si/AI). It can be seen from the analytical results in table 3, that there is a significant amount of organic matter incorporated in the zeolite. A strong signal close to 70ppm
178
on all 13C MAS n.m.r, spectra gives evidence of the presence of the crown-ether ( between 1 and 8 molecules per unit cell). The Rietveld refinement of the crystalstructure of an EMT-type sample showed that each large cage, i.e., both the hypocage and the hypercage contains one 18C6-cation complex [13]. It can be assumed that in the RHO- and KFI-type materials the crown-ether complexes are occluded in the large LTA-type cavities. But according to the chemical analysis only 50 to 70% of these cavities are occupied. In the case of the FAU-type zeolite the occupation factor of the supercage is close to one. The d.t.a.results show that the thermal decomposition of the crown-ether occurs at much higher temperature for the RHO-and KFI-type materials ( between 300 and 380~ than for FAU- and EMT-type materials ( between 160 and 280~ This difference can be related to the size of the apertures which are circumscribed by 8 membered rings in the former and by 12 membered rings in the latter. Table 3 Chemical composition (wt%) of some zeolite samples in their as-synthesized form (a) wt % Sample Struct. SiO2 AI203 Na20 K20 Cs20 SrO H20 Organic species type TG a CA b NMR c A FAU 46.8 14.3 8.6 / / / 17.0 12.4 12.1 n.d. D EMT 52.7 11.8 7.7 / / / 16.5 12.3 12.2 n.d. E RHO 54.4 11.9 5.2 / 10.6 / 12.5 6.0 5.9 5.9 H RHO 57.9 10.6 4.5 / 9.1 0 9.3 9.1 9.0 n.d. I KFI 51.5 12.6 / 12.1 / 1.2 n.d. / / ./ M KFI 57.1 12.8 / 10.3 / 1.2 16.4 3.1 3.1 3.0. (b) Si/AI molar ratios and 18-crown-6 per unit cell Sample Si/AI molar ratio 18-crown-6 CAb NMR d per unit cell A 2.8 3.0 ~8.5 a determined by thermogravimetry b determined by chemical analysis D 3.8 3.7 ~4.0 E 3.9 3.9 ~1.0 c determined by liquid 1H NMR H 4.6 4.6 ~1.4 d determined by 29Si MAS NMR I 3.5 3.6 / n.d. 9not determined M 3.8 4.0 ~1.0 .
.
.
.
3.4. A d s o r p t i o n
measurements An original result is observed for the RHO-type material. Indeed, the n-hexane sorption capacity (Table 4) is high and the corresponding porous volume is equal to 0.26 cm31iq.g-1.
Table 4 Adsorption of n-hexane Sample Structure type D E M
EMT RHO KFI
Adsorption capacity (wt%) 19.5 17.1 13.7
Porous volume (cm31iq.9-1) 0.29 0.26 0.21
179
This value, which is very close to the theoritical one ( 0.33 cm31iq.g -1114].) is larger than that observed for a classical RHO material (prepared in the absence of 18-crown-6), where only 50% of the theoritical volume is accessible [14]. This higher sorption capacity can be related to the non-distorded high-silica RHO framework [7]. 3.5. R e t r i e v a l of 1 8 - c r o w n - 6 e t h e r f r o m E M T z e o l i t e s
Given the high cost of the crown ether molecule, it is particularly relevant to find a procedure leading to the recovery of the intact macrocycle, and possibly allowing further recycling in synthesis. A few studies dealing with the removal of the organic templating agents from molecular sieves without calcining the samples are reported in literature. In 1986 Gelsthorpe and Theocharis [15] succeeded in extracting triethylamine from AIPO4-5 and SAPO-5 by treating these materials with a solution of methanol and hydrochloric acid at 243~ This method was further used and extented to other porous aluminophosphates by Malla and Komarneni ([16]. The EMT-type zeolite samples were treated in autoclaves by using various solutions as shown in Table 5. Table 5 Extraction media and yields (%) (extraction conditions" liquid/solid ratio 5-50, salt concentration 1-3 mol.I -t, pH 3- 7) Extraction medium Extraction yields (%) Solvent alone H20, C1 -C4 alcohols 15- 40 Solutions of salts of small cations Solutions of salts of large cations
e.g., K+, NH4 +. -protonated amines: e.g.,Et2NH, Et3N, Pr3N -quaternary ammonium salts: e.g., Me4N+ , Et4N+
30- 60 60- 95
According to the nature of the extraction medium, three extraction levels were reached: - with a solvent alone (H20 or alcohols from C1 to C4 or H20-alcohols mixture), the extraction yields did not exceed 40%. - with a solution containing small cations like alkaline or ammonium cations, the yields increase to 60%. - with a solution containing large cations like protonated amines or quarternary ammonium cations, almost all the crown-ether could be extracted. This is in agreement with the conditions which have to be fulfilled by extraction medium: it has to be a good solvent for the crown-ether or its cationic complex and it has to replace in the zeolite,with similar interaction, the extracted ether or its cationic complex.Thus water or alcohols are good solvents for the crown ether, but as guests in the silica-rich zeolite their interaction with the sodium cations is weaker than for the crown-ether. The presence of cations in the solvent helps probably the extraction because the crown-ether is stabilized in solution in the form of complexes. Moreover there can be a simultaneous cation exchange. When the cations present in the zeolite after exchange are similar to the sodium cations, this exchange does not improve the extraction. Only when the new cations exhibit stabilizing interactions
180
and volumes comparable to those of the crown-ether cation complexes, the exchange has a beneficial effect on the extraction. This is the case of bulky and relatively hydrophobic alkylammonium cations which seem to be the most suitable to mimic the 18C6-Na + complex. Among those the protonated triethylamine led to the highest extraction yield (95%). 4. CONCLUSION
FAU-, EMT-, RHO- and KFI-type zeolites were prepared by using the 18-crown-6 ether in an aluminosilicate gel composition. The addition of such an organic species to the starting mixture brought about some significant improvements. The first of them is purity since in a completely inorganic medium usually unwanted by-products appeared. Moreover, until now, the EMT structure-type cannot be obtained, even as traces, in the absence of 18-crown-6. The second outcome was a better crystallinity of the desired products. The use of the crown-ether molecule also resulted in an increased framework Si/AI molar ratio. This result can be related to the fact that the crown-ether is always incorporated and acts as a specific stabilizing template 5. ACKNOWLEDGEMENTS
The authors would like to thank Dr. H. Kessler for fruitful discussions and S. Einhorn for taking the photographs. Financial support of this work was provided by the European Union (Brite Euram program). REFERENCES
1. 2. 3. 4.
F. Delprato, L. Delmotte, J.L. Guth and L. Huve, Zeolites, 10 (1990) 546. S.L. Burkett and M.E. Davis, Microporous Materials, 1 (1993) 265. C. N. Wu and K. J. Chao, J. Chem. Soc. Farad. Trans., 91 1 (1995) 167. E.J.P. Feijen, K. de Vadder, M.H. Bosschaerts, J.L. Lievens, J.A. Martens, P.J. Grobet and P.A. Jacobs, J. Am. Chem. Soc., 116 (1994) 2950. 5. T. Des Couri~res, J.L. Guth, J. Patarin and C. Zivkov, U.S. Pat.5 273 945 (1993). 6. T. Chatelain, J. Patarin, M. Soulard, J.L. Guth and P. Schulz, Zeolites, 15 (1995)90. 7. T. Chatelain, J. Patarin, E. Fousson, M. Soulard, J.L. Guth and P. Schulz, Microporous Materials, 4 (1995) 231. 8. J.P. Verduijn, U.S. Pat. 4 944 249 (1990). 9. American Society of Testing Materials, ASTM Designation D 3906-85a (1985). 10. F. Dougnier, J. Patarin, J.L. Guth and D. Anglerot, Zeolites, 12 (1992) 160. 11. D. Anglerot, F. Fitoussi, P. Schulz, T. Chatelain, F. Dougnier,J. Patarin and J.L. Guth, ACS meeting, Anaheim 1995, accepted. 12. M.M.J. Treacy, J.M. Newsam and M. W. Deem, Proc. Roy. Soc. Ser. A, 433 (1991 ) 499. 13. C. Baerlocher, L.B. McCusker and R. Chiapetta, Microporous Materials, 2 (1994), 269. 14. W.H. Flank, ACS Symp. Ser., 40 (1977) p.43. 15. M.R. Gelsthorpe and C.R. Theocharis, J. Chem. Soc., Chem. Commun., (1986) 781. 16. P.B. Malla and S. Komarneni, Zeolites, 15 (1995) 324.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
181
Synthesis of zeolites in a microwave heating environment Jing Ping Zhao, Colin Cundy and John Dwyer Centre for Microporous Materials, Department of Chemistry, UMIST, P.O. Box 88, Manchester M60 1QD, UK
ZSM-5, zeolite /3 and hexagonal Y (EMT), are successfully synthesised using microwave heating. NH 4 form [Ti]ZSM-5 and [A1]ZSM-5 are also obtained under microwave heating conditions in the presence of fluoride anions. NaY can be very rapidly crystallised in the microwave environment. High temperature (150 ~ C) can be used in NaY synthesis without inducing crystalline impurity, demonstrating the tendency of the microwave procedure to provide and maintain phase purity under favourable conditions. By comparison with conventional heating, microwave methods can significantly shorten the overall nucleation and crystal growth periods for most of the zeolites investigated, but the effect is greater in some cases than in others. In a microwave environment, a higher temperature can often be used in zeolite synthesis to gain extra benefits.
1. INTRODUCTION Zeolites are usually synthesised under hydrothermal conditions in a period from a few hours to a few days depending on the nature of the zeolite, mixture composition and the synthesis temperature. Frequently, low temperatures must be used to reduce the formation of undesired phases. However, working at a low temperature necessitates longer synthesis times which may prove too costly or impracticable for industrial application. Therefore, reducing the crystallisation time may be one of the most important targets for commercial synthesis. Recent research shows that microwave techniques present new possibilities for achieving such a target [1,2]. This paper examines the syntheses of various zeolites under microwave heating conditions and discusses the possible contribution of microwave energy to the formation of zeolites. [AI]ZSM-5, zeolite/3, EMT (Hexagonal Y) and NaY have been prepared using hydroxide ion as mineraliser. NH4 form [Ti]ZSM-5 and [A1]ZSM-5 are also synthesised from mixtures containing fluoride anion. By comparison with a conventional heating system, microwave heating can significantly reduce overall crystallisation time. It is also observed in the synthesis of Na-Y that microwave heating can significantly accelerate the formation of the FAU structure, and with a much reduced occurrence of P-type (GIS) impurity. Because of this "preference" or "selectivity", a higher temperature can be applied in NaY synthesis, making the process faster and potentially more cost effective.
182 2. EXPERIMENTAL The raw materials used were sodium aluminate (AlzO3=32.75 %, NazO=28.5%, BDH), NH4F (BDH), NaF (BDH), NaOH (BDH), 18-Crown-6 (BDH), Tetrapropylammonium bromide [TPABr] (Aldrich Chemicals), Silica sol (Ludox AS 40, SiO2=40%, Aldrich Chemicals), Fumed silica (BDH), Tetraethyl-ammonium hydroxide (20% solution, Aldrich) and TIC13 (BDH). The microwave equipment used in this work was a CEM MDS-2100 sample preparation system using a fibre optic temperature controller and a pressure controller and an adjustable power output (maximum 950W at 2450 MHz). Teflon PFA autoclaves (100 ml, unstirred), were used. The samples synthesised were characterised using 295i MAS N M R , XRD, SEM and EDAX.
3. RESULTS AND DISCUSSION 3.1 [Ti]ZSM-5 and [A1]ZSM-5 [A1]ZSM-5 was synthesised from reaction mixtures of composition xNa20-yA120360SiO2-zTPABr-nHaO, where x=4.5-7, y=0-2, z=4-8 and n=800-1600, prepared according to the following procedure. First, a silica-containing mixture (mixture A) was made by mixing silica sol (Ludox) and template (TPABr) with 1/3 of the total water. Secondly, mixture B was prepared by mixing NaA102 and NaOH with a further 1/3 of the calculated water. Both mixtures were stirred for 30 minutes. Finally, mixture B was slowly added to mixture A with vigorous stirring and the reaction gel was continuously stirred for 2 hours. The final composition was then transferred into autoclaves and heated by microwave. The temperature was controlled by a programme which in essence contains two stages which are D E temperature elevation and C temperature maintenance. The first stage usually takes 1-2 minutes and the A B second stage depends on the reaction temperature and mixture composition. 5 15 25 35 5 Twotheta Using a reaction mixture with a typical composition 5.0NazO-0.2AlzO3-60SiOz- Figure 1. XRD patterns of [A1]ZSM-5 synthesised from 4.0TPABr-900H20, a an alkaline system under microwave heating. very crystalline ZSM-5 A) 1.65 h B) 2.0 h C) 2.35 h D) 2.65 h E) 3.0 h
183 can be obtained at 170~ without seeding in 2-3 hours (Figure 1). The XRD patterns of the [A1]ZSM-5 show that the nucleation takes less than 1.65 hours and the crystal growth needs only about 1 hour. This demonstrates that [A1]ZSM-5 can be synthesised very rapidly from a conventional reaction mixture using microwave heating. The particle size of the [A1]ZSM-5 is 3-4 25 35 45 5 15 ~tm and no TwoTheta crystalline impurity phases are observed. Figure 2. XRD patterns of [A1]ZSM-5 synthesised from a In order to fluoride system under microwave heating. study the effects of 1) 7.0 hours; 2) 8.0 hours 3) 9.0 hours microwave heating on a different synthesis system, the method based on fluoride anion was chosen. The reaction mixtures were prepared using reported procedures [3,4]. Two typical reaction mixtures were used to study the effects of microwave energy on the formation of [Ti]ZSM5 and [A1]ZSM-5 in the presence of fluoride anions. Their compositions were 1.0NH4F0.03TiCI3-1.0SiO2-0.5TPABr-30H20 and 2.0NH4F-0.14A1C13-1.0SiO2-0.5TPABr-30H20. Both used silica sol (Ludox AS 40) as silica source. The reaction mixtures are usually aged overnight, but such a step is not essential. On microwave I ~ l heating, the MFI structure can be detected by XRD from the reaction mixtures after about 5 15 25 35 Two "Fheta 45 6-7 hours at 170~ C. The crystallisation will then take a Figure 3. XRD patterns of [Ti]ZSM-5 synthesised from a fluoride further 1-2 hours to system under microwave heating, complete. The XRD 1) 7.0 hours 2) 8.0 hours 3) 9.0 hours !
184 patterns of NHa-[AI]ZSM-5 and NH4-[Ti]ZSM-5 are given in Figure 2 and Figure 3 which show that they are both very good crystalline products. As can be seen the nucleation takes about 7 hours and the crystal growth needs only about 1.5 hours which is similar to that in an alkaline system. This suggests that microwave energy has no unique influence on the crystal growth in either the fluoride or in the alkaline synthesis system. It is also appearent that nucleation is the major factor controlling the overall crystaUisation time of the MFI structure in the fluoride system. Under conventional heating, the crystallisation takes about 20 hours at 175~ C using comparable reaction compositions [4], demonstrating an effective acceleration of 2-3 times using the microwave method.
3.2 Syntheses of zeolite/3 and hexagonal NaY (EMT) Zeolites 13and EMT can also be synthesised in a microwave heating environment. For zeolite/3, the reaction mixture was prepared by adding a solution containing NaA102 and NaOH to a mixture of fumed silica and TEAOH. A seeding slurry was then B optionally added. The final mixture was aged at room temperature overnight. The seeding slurry has a similar composition to the main reaction mixture but has been pre-heated 5 1~5 25 35 in a conventional oven Two Theta to nucleate. In the seeding slurry, zeolite XRD patterns of zeolite/3 synthesised at 140~ /3 can be detected using Figure 4. under microwave heating. XRD analysis. A A) 10 hours B) 14 hours typical reaction mixture has the composition 2.5Na20-1.0A1203-40SiO2-6.0(TEA)20-560H20. Usually, the amount of seeding slurry is between 4 % and 8 % based on SiO2 + A1203 in the mixture. Figure 4 gives the XRD pattern of the product after 14 hours microwave heating at 140~ C. The wellcrystallised zeolite has a Si/A1 ratio of 14 as measured by 29 Si NMR spectroscopy. Hexagonal Y (EMT) is one of most difficult aluminous zeolites to synthesise, normally taking 4-12 days at 110~ C by conventional heating [5]. However, it can be obtained in one day using microwave energy by working at a higher temperature. The composition of synthesis mixture was 2.4Na20-0.5NaF-(0.85-1.0)A1203-10SiO2-(0.5-0.8)[18-Crown-6]140H20, prepared as described previously [5]. At a lower temperature (110 ~ C), EMT can be detected after microwave-induced crystallisation for about 1.8 days and the crystal !
!
185 growth takes a further 2 days, which is nearly as long as in a conventional hydrothermal synthesis at that temperature. It is clear that the crystallisation of the EMT under these conditions is very difficult. When a higher temperature ( 115~ C) is used, a very crystalline EMT can be obtained in about 2.5 days (Figure 5). The c fast increase of crystallisation with a very small rise in temperature may suggest that the formation of EMT is very sensitive to temperature in a microwave environment. With further increase of ! 0 1~0 20 Two Theta 30 40 the temperature (130150~ C), EMT can be obtained between 820 hours depending Figure 5. XRD pattern of EMT synthesised without seeding on the reaction under microwave heating. t e m p e r a t u r e . A) 3.0 days at 110~ B)l.8 days at 115~ C)2.5 days at 115~ However, small amounts of amorphous or other impurity phases are generally unavoidable. If a seeding technique similar to that used in standard zeolite Y synthesis is used, the purity of the product can be improved, particularly at a higher temperature (150~ C).
3.3 NaY synthesis Highly crystalline NaY was synthesised in a very short time using microwave heating. The reaction mixtures were prepared by adding a solution of NaA102 and NaOH to a diluted silica sol. The compositions employed were xNazO-1.0A1203-ySiO2-240H20 , where x=4-7 and y = 10-20. When y = 10 and x=6.2, a very crystalline NaY can been obtained at 110~ in less than 1.5 hours under microwave heating without seeding. Using the same reaction mixture, the synthesis takes 9-10 hours at the same temperature under conventional heating conditions in order to achieve a good crystalline product. The synthesis time is about 6 times shorter using microwave heating. Zeolite P is an impurity phase frequently obtained in conventional NaY preparations, usually rendering NaY production impossible at higher temperature. Therefore, most industrial processes use a lower temperature (usually ca. 100~ At this temperature, the crystallisation usually takes from 10 to 30 hours. In order to study the formation of zeolites at different temperatures in a microwave environment, the NaY synthesis system was chosen. It is found that, using microwaves,
186 there is far less conversion to P-type zeolite even at higher temperatures (150 ~ C). At such a high temperature, formation of P-type zeolite is usually unavoidable by conventional heating. For example, heating the same reaction mixture at 150~ C by conventional means, produced a P-type zeolite resembling Gobbinsite [6] without any NaY. At 150~ C, the FAU structure can be detected by XRD after about 5 minutes microwave heating and the crystal growth takes a further 10-15 minutes (Figure 6). The crystalline product had an average crystal size of about 0.5-1.0/~m without any detectable crystalline impurity. Continuing the microwave heating for a total of 120 minutes yielded no evidence of any other crystalline phase. This suggests that microwave energy has made an effective and apparently selective contribution to the formation of the FAU structure D which is also stable in the microwave C reaction environment. Again, it appears that the use of B microwave /" energy may have a particular , , i 310 i advantage in 0 lb ' 2'0 Two Theta 40 encouraging the .
.
.
.
.
.
_
_
,
:
.
.
.
.
.
_
-
7
nucleation of a Figure 6. XRD patterns of NaY synthesised at 150 ~ C without s in g 1e p h a s e seeding under microwave heating. under favourable A) 5 min. B) 10 min. C) 15 min. D) 20 min. conditions rather than exerting any unique influence upon crystal growth. The effect of microwave heating on the synthesis of high-silica NaY has also been studied. When Na20=5.8 and SiO2 = 15, a very crystalline NaY can be obtained in less than 1.5 hours, with seeding, at 150~ C. A typical product had SiO2/AlzO 3 = 4.7 as calculated from the unit cell parameter [7]. This demonstrates that a fairly siliceous NaY can also be obtained very rapidly at a higher temperature without crystalline impurity. Unfortunately, the true comparison of microwave heating with conventional heating at higher temperatures cannot be made because pure NaY cannot be obtained from oven-heated autoclaves under these conditions.
4. CONCLUSIONS The syntheses of [AI]ZSM-5 and [Ti]ZSM-5 can be accelerated in a microwave heating environment without seeding using either traditional alkaline media or in the presence of fluoride ions. With microwave heating, [A1]ZSM-5 can be obtained from a normal OH-
187 based composition in 2.5 hours. In most cases, crystaMsation can be speeded up by 2-3 times by using microwave heating as compared with conventional heating. Very crystalline zeolite/3 can be crystallised in 14 hours from the standard NaOH/TEAOH system using microwaves. Highly crystalline EMT can similarly be obtained at 115~ in 2.5 days without seeding. The formation of EMT is very sensitive to the synthesis temperature. The most notable contribution so far observed for microwave energy input is found in NaY synthesis. By using microwave heating, under given conditions, a reduction in overall synthesis time of up to 6 times can be achieved compared to conventional methods. NaY can be crystallised in times ranging from 10 minutes to 1.5 hours depending on the composition of the reaction mixture. In NaY synthesis, it is found that for approximately every 15 degree increase in reaction temperature, the crystallisation time is reduced by a half. Microwave heating can use this to advantage by limiting the formation of impurity phases (particularly zeolite P) and providing, in effect, selectivity towards NaY. A much higher temperature can therefore be applied in microwave-mediated NaY synthesis than in conventional synthesis procedures. Consequently, there is considerable scope for the improvement of existing procedures in terms of time and cost and perhaps also for the development of new continuous processes.
ACKNOWLEDGEMENTS We thank the EPSRC for their financial support (GR/K06877) of this work and R J Plaisted for helpful discussions.
REFERENCES 1. 2. 3 4. 5. 6. 7.
A. Arafat, J. C. Jansen, A. R. Ebaid and H. van Bekkum, Zeolites 13 (1993), 162-5. P. Chu, F. G. Dwyer and V. J. Clarke, Eur. Pat. 358 827 (1990). J. Zhao, J Dwyer and D Rawlence, Proceedings of the 9th International Zeolite Conference. Montreal (1992), 155-61. J. Zhao and J. Dwyer, paper in preparation. K. Karim, J. Zhao, D. Rawlence and J. Dwyer, Microporous Materials, 3 (1994) 695-698. R. von Ballmoos and J. B. Higgins, Collection of Simulated XRD Powder Patterns for Zeolites, Zeolites, 10(5), (1990). D . W . Breck, Zeolite Molecular Sieves, Wiley, New York, p49, 1974.
This Page Intentionally Left Blank
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
SYNTHESIS OF OCTAHEDRAL
MOLECULAR
189
SIEVES
Chi-Lin O'Young' and Steven L. Suibb 'Texaco Inc. P.O. Box 509, Beacon, NY 12508 USA ~Dept. of Chemistry~ U. of Connecticut, Storrs, CT 06269-3060 USA A large number of families of manganese oxide octahedral molecular sieves (OMS) and their precursors, octahedral layered materials (OL), have been synthesized and characterized by various methods. The materials include OMS-1, OMS-2, and OL-1; they all use MnO6 octahedra as the basic structural unit to form (3X3) tunnels, (2X2) tunnels, and layered structures, respectively. Different metal cations can incorporate into the OMS and OL structures through framework, tunnel, and interlayer substitutions. These materials can be synthesized by the reflux, hydrothermal, precipitation, calcination, ion-exchange, isomorphous substitution, and sol-gd methods. The materials have been characterized in detailed by a variety of techniques to study the structure, composition, stability, and morphology. This paper will discuss and review the different methods used to synthesize OMS and OL materials and the resultant changes in physical and chemical properties. 1. INTRODUCTION Synthesis of novel zeolites and molecular sieves such as intersecting 10- and 12-ring pore zeolites [1] and mesoporous materials [2] have been a major focus of several research groups in the past few years. Unique structural materials that result in porous and open l~amework systems such as vanadium phosphates with 18.4 A tunnels [3] and porous TiO2 materials [4] are continually being discovered. The synthesis, characterization, and applications of todorokite [5] and cryptomelane (or hollandite) materials [6-8] have been reported. These OMS materials use MnO~ octahedra as the basic structural unit to form mono-directional tunnel structures. The synthetic todorokite (OMS-1) and cryptomelane (OMS-2) have (3x3) and (2x2) tunnels with pore sizes of 6.9 x 6.9 A and 4.6 x 4.6 A, respectively (Figure 1). The precursors of OMS, bimessites or octahedral layered materials (OL-1), consist of layers of edge and comer linked MnO6 octahedra with water molecules and metal cations in the interlayer voids and have an interlayer distance of 7 to 10 A. Certain metal cations can incorporate into the OMS and OL structures through framework, tunnel, and interlayer substitutions [7,9]. The framework substitutions of OMS and OL are represented as [M]-OMS and [M]-OL, while the tunnel and interlayer substitutions are represented as M-OMS and M-OL, respectively. These OMS and OL materials can be synthesized by the reflux, hydrothermal, precipitation, calcination, ion-exchange, isomorphous substitution, and sol-gel methods and result in materials that
190 have different physical and chemical properties. We will discuss and review these various methods used to prepare OMS and OL materials and resultant changes in physical and chemical properties.
OMS-1 Todorokite
OL-1 Birnessite
. . . . .
H20
G
~
9
G
~
|
.,
OMS-2 Hollandite
.....o
M n+
9
9
r//.
.
Mn2~ Co2§ , Ni2§ Cu 2., Zn2§
(sx3)
(2xe)
Cd 2+, Mg2+ Figure 1. Structure of OL-1, OMS-1, and OMS-2 T.~...b.Le..~..~.~.~.m.~!.~...?.f..~s...~..~..~L~.~..a.t.e.~..gr..e.p...~.r.e...~....~r.~y.~..d?...".t..~rth.~.~.
Structure 1. K-OMS-2
Reactants KMn04, MnSO,
2. K-OMS-2 3. K-OMS-2 4. K-OMS-2 5. M-OMS-2 6. [M]-OMS-2
12. Mg-OMS- 1
KMn04, MnSO4 K-OL-1 from #8 KMnO4,maleic acid K-OMS-2 form # 1, 2 # 1, 2 & dopants added to initial solution MnCI2, NaOH, Mg0VlnO4)2 MnSO4, KOH, 02 KMnO4, sugar Na-OL- 1 from #7 #7 & dopants added to initial solution Mg-OL- 1 from # 10
13. M-OMS- 1
M-OL-I from #I0
14. [M]-OMS- I
[M]-OL- I from # I I
7. Na-OL-1 8. K-OL-1 9. K-OL-1 10. M-OL- 1 1 !. [M]-OL-1
............................................................................................................
.............................................
Method/Conditions Hydrothermal, autoclave 100 ~ 17 h, low pH's Reflux 100 ~ 17 h, low pH's Calcination, 600 *C, 17 h Sol-gel, 450 *C, 4 h Ion-exchange Isomorphous substitution, reflux or hydrothermal Precipitation, 25 ~ aging, high pH's
Precipitation, 25 ~ high pH's Sol-gel, 450 ~ 2 h Ion-exchange, 25 ~ Isomorphous substitution, 25 ~ aging, high pH's Hydrothermal, autoclave 175 *C, 20 h Hydrothermal, autoclave 175 ~ 20 h Ion-exchange, hydrothermal, ~.t..o..~ay~..!.7...5....*...C..,...~O.~
References 6
7 7 8 7 7 5 7 10 5, 9
5 9
.........................................................................
191 2. EXPERIMENTAL SECTION Table 1 shows fourteen families of OMS and OL materials have been prepared by the reflux, hydrothermal, precipitation, calcination, ion-exchange, isomorphous substitution, and sol-gel methods.
2.1. Synthesis of OMS-2 with (2X2) Tunnel Structure K-OMS-2 have been synthesized by the hydrothermal [6], reflux [7], calcination [7], and sol-gel [8] methods (Methods 1 - 4). A typical hydrothermal or reflux synthesis was as follows: 100 mL of 0.4 M KMnO4 was added to a mixture of 30 mL of 1.74 M MnSO4 and 3 mL of concentrated HNO3. The final mixture was autoclaved or refluxed at 100 *C for 17 h; the product was filtered, washed, and dried. A standard calcination preparation was as follows: 200 mL of 3.12 M KOH was added to 200 mL of 0.89 M MnSO4. Oxygen was bubbled (12 L/min) through the solution for 4 h. The black product was filtered, washed, and calcined at 600 *C for 17 h. A typical sol-gel preparation was as follows: 3 m mole of maleic acid was added to 100 mL of 0.1 M KMnO4 and the mixture was stirred for 30 min. A dark brown sol was formed at room temperature which started to gel in 30 rnin. The resultant gel was filtered, washed, and calcined at 450 *C for 4 h. The tunnel substitution of K-OMS-2 was prepared by the ion-exchange method (Method 5) [7]. The framework substitution of K-OMS-2 was prepared by adding metal dopants (a total concentration of 0.01 M) into the initial solution, followed by reflux or autoclave treatment as described before (Method 6) [7]. 2.2. Synthesis of OL-I The precursor of OMS-1, Na-OL-I, was prepared by reacting MnCl2 with NaOH to form pyrochroite, Mn(OH)2, followed by adding a solution of Mg(MnO4)2 to the suspension to form NaOL-1 (Method 7) [5]. KMnO, or NaMnO, also could be used to prepare the same quality of precursor by adding an equivalent amount of Mg 2+ into the mixture. A typical preparation was as follows: 50 mL orS.0 MNaOH solution was added to a mixture of 40 mL of 0.5 M MnCl2 and 0.1 M MgCl2 in a plastic bottle with stirring. 40 mL of 0.2 M KMnO4 or NaMnO4 was then added to the suspension. The mixture was aged at room temperature for 7 days. The precipitate was filtered and washed thoroughly with water. XRD of the wet precipitate showed peaks at 10.1, 5.0, and 3.33 A. The interlayer peak shined from 10.1 to 7.1 Jk after drying. MgCl2 also could be mixed with the KMnO, or NaMnO4 solution, and the results were the same. The precursor of OMS-2, K-OL-l, was prepared by reacting MnSO4 and KOH with oxygen bubbling through the solution as described previously (Method 8) [7]. The sol-gel K-OL-1 was prepared by reacting KMnO4 and simple sugars (glucose or sucrose) to form a brown gel, followed by drying and calcining at high temperatures (Method 9) [10]. A standard preparation was as follows: 50 mL of 0.38 M KMnO4 was added to 20 mL of 1.4 M glucose to form a brown gel, and the gel was then washed, dried, and calcined at 450 *C for 2 h. The interlayer substitution of Na-OL-1 was prepared by the ion-exchange method at room temperature (Method 10) [9]. For the l~amework substitution, [M]-OL-1 was prepared by adding metal dopants (6 mL of 0.1 M metal salts) into the initial solution as described previously (Method
II).
192 2.3. Synthesis of OMS-I with (3X3) Tunnel Structure Mg-OMS-1 was prepared by the rearrangement of Mg-OL-1 under hydrothermal conditions (Method 12) [5]. The tunnel substitution of OMS-1 was prepared by the ion-exchange of Na-OL-1 with metal ions (Method 10), and consequently convened to M-OMS-1 by the hydrothermal treatment (Method 13) [9]. The fiamework substitution of OMS-1 was prepared by adding metal dopants into the initial solution to form [M]-OL-1 (Method 11), followed by the ion-exchange with Mg2§ then converted to [M]-OMS-1 by the hydrothermal treatment (Method 14). 2.4. Characterization Techniques Various characterization techniques have been applied to study the structure, composition, morphology, and thermal stability of these materials. They included X-ray powder diffraction (XRD), microanalysis, transmission electron microscopy (TEM), scanning electron microscopy (SEM), thermal analysis, temperature programmed desorption (TPD) and reduction (TPK), cyclic voltammetry (CV), and others. Details of the procedures have been disclosed in the literature [512].
3. RESULTS 3.1 Synthesis The hydrothermal and reflux preparations of K-OMS-2 involved reactions between MnO4" and Mn2§ solutions. The size and concentration of counter cation, pH, and temperature were identified as important preparation parameters. The optimal conditions are: pH's < 2, 80 to 140 ~ and [KMnO4]/([KMnO4] + [Mn2"]) > 0.4. The template effects of counter cations were clearly observed in both methods [6,7]. The calcination method involved the heat treatment of the layered precursor, K-OL-1, at 6OO~ The sol-gel method involved reactions between KMnO4 and pure maleic acid. The critical preparation parameters included the concentration of permanganate, nature of the counter cation and the organic acid reducing agent, temperature of gelation and calcination. A mixture of OMS-2 and OL-I was formed if the concentration of permanganate was too high (0.35M). KMnO4 and CsMnO4 yielded most crystalline and thermally stable (800 oC) sol-gel OMS-2. NaMnO4, LiMnO4, Ca(MnO4)2, and Mg0VInO4)2leaded to less stable and impure products. The optimal conditions are: a concentration of KMnO4 around 0.1 M, pure and flesh maleic acid, reaction temperature around room temperature, and calcination temperature around 400 ~ [8]. Several critical parameters for the synthesis of Mg-OMS-1 and the precursor, Na-OL-1, were identified; they included the pH, ratio of MnO4" to Mn2§ Mg2+concentration, time and temperature of aging, time and temperature of autoclaving. The optimal conditions for the synthesis of OMS-1 are: a MnO4"/Mn2§ ratio of 0.3 to 0.4, pH of 13.8, aging at 25 to 35 ~ for 1 to 7 days, and autoclave treatment at 160 to 180 oC for 4 to 7 days. The effects of pH, MnO4"/Mn2+ ratio, and autoclave conditions have been discussed in the literature [5]. The crystaUinity and thermal stability of OMS-1 strongly depended on the crystallinity of the precursor. Table 2 shows the effects of aging temperature (5 to 35 *C) and time (1 to 7 days) on the crystallinity of Na-OL-1. The integrated intensity of the d(001) peak at 10.1 A was measured and used as an index of the crystaUinity. The results show that the crystallinity of Na-OL-1 is quite sensitive to the aging time and temperature. For example, aging at 35 *C for 1 day has about the same crystallinity as aging at 5
193 oC for 7 days. Aging at higher temperature (80 *C) significantly increases the crystallinity; however, the resultant Na-OL-1 loses the ion-exchange capacity and cannot form Mg-OL-1 and OMS-1. Table 2. Effects of aging time and temperature on crystallinity of Na-OL-I Aging Temperature Aging Time ~ Days 5 20 5941 9050 1 7345 11100 2 11982 14700 4 13069 15170 7 Values are the integrated intensity of the d(001) peak at 10.1 K
35 13571 16254 22100 24486
The Mg2§ concentration is another important preparation parameter. The most crystalline and thermally stable OMS-1 materials are prepared by Mg(MnO4)z. Using NaMnO4 or KMnO4 yields less stable and impure products. However, the same quality of OMS-1 can be formed when an equivalent amount ofMg 2+is added into the initial solution. For the sol-gel synthesis of K-OL- 1, the counter cation of permanganate plays an important role in reactions of MnOi with sugars. Different cations influence both gel formation and the nature of the final product. Only KMnO, yields sol-gel and pure products; NaMnO4 and Mg(MnO,)2 do not produce sol-gel K-OL- 1 products [ 10]. 3.2 Ion Exchange Properties K-OMS-2 prepared by the reflux and hydrothermal methods exhibit some ion-exchange properties. At room temperature, about 70% of tunnel K§ can be exchanged with Rb§ Li§ and Na + cannot exchange K § easily [7]. At 80 *C, K-OMS-2 can be exchanged with NH4+, Co2+, Cu2+, and Ni2+to form tunnel substituted [M]-OMS-2. The percentage of exchange capacity shows the order: NI-I4+ (36%) > Co2§ (18%) > Ni 2+(5.8%) ~ Cuz+(4.4%). Na-OL-1 prepared by Method 7 has very good ion-exchange capacity when it is wet. However, dehydration of Na-OL-1 decreases the interlayer distance from 10.1 to 7.1 ~ and loses the ionexchange capacity. Mg 2§ Ni2+, Co2+, Cu2+, and Zn2+ can be exchanged easily at room temperature with wet Na-OL-1 to from M-OL-1 and consequently converted to M-OMS-1 under the hydrothermal conditions [9]. Direct ion-exchange of Mg-OMS,1 to form tunnel substituted MOMS-I has not succeeded. Sol-gel K-OL-1 doesn't have any ion-exchange capacity at room temperature. 3.3. Framework Substitution The isomorphous substitutions of cations intothe OMS and O L l~amework structures involved addition of metal dopants into the solution precursors prior to any precipitation or reaction. A variety of cations, such as Cr~§ Fe3+, Co2§ Ni~§ Cu2+, and Zn2+ have been incorporated into the OMS-2 framework. At 0.01 M of dopant concentration and the standard conditions, the degree of substitution was between 1.5% to 1.7%. Divalent cations with ionic diameters similar to Mn2§ such as Mg 2§ Co2§ Niz§ Cuz§ and Zn2§ have been incorporated into the framework of OMS-1 by Method 14. Results of compositional
194 analysis showed that all doped cations (about 2%) were totally retained in the corresponding OMS1 materials. 3.4 Characterization K-OMS-2 prepared by the four different methods all have the same XRD patterns; however, they have quite different properties of crystaUinity, thermal stability, and morphology (Table 3). The reflux, autoclave, and sol-gel materials have higher average manganese oxidation states than the calcination material. XRD of the calcination and sol-gel materials show sharper peaks than those of the reflux and autoclave materials. The reflux and autoclave materials are thermally stable up to 600 ~ whereas the calcination and sol-gel materials are stable up to 800 *C. The morphology of the reflux and autoclave materials are needle-like; however, the morphology of the calcination and solgel materials are clump and irregular. Temperature programmed desorption (TPD) data for 02 evolved show that the reflux and autoclave materials have much higher oxygen loss than the sol-gel material. Table 3. Comparison of OMS-2 prepared by Reflux, Autoclave, Calcination, and Sol-Gel Methods Parameter Reflux Autoclave Calcination Sol-Gel broad broad sharp sharp XRD 3.80 3.96 3.68 3.80 Ave. Mn Oxidation state 600 ~ 600 ~ 900 ~ 800 ~ Thermal Stability needles needles clumps irregular SEM 9.41 of16 O 9.41 of16 O N.A. 0.48 of16 O Oxygen Desorption (TPD)
Tunnel cations have profound effects on the thermal stability and morphology ofM-OMS-1 [9]. Results of TGA and XRD show that Mg-OMS-1 is thermally stable up to 600 ~ Co-OMS-1 and Ni-OMS-1 are stable to 500 ~ and Cu-OMS-1 and Zn-OMS-1 are stable to 300 *C. SEM results show that the crystal morphologies of M-OMS-1 can be plates, needles, or fibrous shapes, depending on the nature of the cations. TPD results show that the tunnel cations do not markedly affect the evolution of TPD peaks, but remarkably influence TPR in both H2/Ar and CO/He with respect to both emerging temperature and population. Cu-OMS-1 appears to process more oxygen species that are especially reactive with 1-12and CO at low temperatures [ 11]. Results of XRD and TGA show that framework substituted [Zn]-, [Co]-, [Ni]-, and [Cu]OMS-1 are all thermally stable up to 400 ~ which are different from the tunnel substituted OMS1. The strongest evidence for fi-amework substitution comes from cyclic voltammetry measurements [12,13]. Results of CV studies show Cu2§ migration out of the OMS-1 tunnels for Cu-OMS-1 with most Cu 2§ in the tunnel, while no such Cu2§ migration is found for [Cu]-OMS-1, indicating the existence of Cu2§ in the framework. Results of electron paramagnetic resonance (EPR) and X-ray photoelectron spectroscopy (XPS) also indirectly support the framework substitution [ 13]. 4. DISCUSSION OMS-1 and OMS-2 have very similar tunnel structures; however, they are synthesized by quite different methods and conditions. Scheme 1 shows two different preparation routes to OMS. Both routes involve redox reactions between MnO; and Mn2+ at different pH's. Low pH's are used for
195 Route 1 tO form OMS-2. XRD of the flesh precipitate shows an amorphous phase. OMS-2 is formed by selecting suitable templates and temperatures. K§ is the major template for the synthesis of OMS-2. Attempts to synthesize OMS-1 by using larger templates are not s u ~ . High pH's are used for Route 2 to form OL-1 as precursors to OMS. XRD of OL-1 prepared by this route show either 10 or 7 A layered phases. However, the critical preparation parameters and conditions for the precursors of OMS-1 and OMS-2 are different. OMS-1 prepared by NaMn04, KMn04, or oxygen [14] are less thermally stable and impure. The effects of Mg2+suggest that a small amount of Mg2§ is in the ~ o r k of layered precursor and OMS-1, which stabilizes the OMS-1 structure. Mg2§ is the major template for the synthesis of OMS-1. K+ and high temperature are essential for the formation of OMS-2 by this route (Method 3). The rearrangement of layered silicates to mesoporous ahminosilicates also has been reported [2]. Scheme 1. Two Different Preparation Routes to OMS
Route 1:
Route 2:
Mn 2+ + MnO4
Mn 2+ +
MnO4 or Oxygen
Low pH's -"
Amorphous Phase
Hi pH's
Temperature ~ OMS-2 Template
Temperature ,~- OL-I
P
Template
OMS-I and
OMS-2
The synthesis" of OMS with (2X5) tunnel structure has been reported in the literature [16]. It was prepared by reacting pyrolusite, (1X 1) tunnel structure, with RbOH solution in a gold capsule under hydrothermal conditions at 350 ~ and 200 Mpa. Another known OMS structure with (2X3) tunnel structure, psilomelane, has not been synthesized. It is still not clear why so different procedures and conditions are needed to synthesize these OMS. Sol-gel methods for the preparation of OMS and OL materials provide several advantages, such as easy incorporation of dopants and template agents directly into the sol. Preparation of thin films via spin coating techniques that might be used in electrochemical or sensor application are also possible. The sol-gel synthesis involves reactions between MnO4" and organic reducing agents. KOL-1 prepared by the sol-gel method is very stable compared to the OL-1 materials prepared by the precipitation, hydrothermal treatment at 160 ~ for 2 days or calcination at 800 ~ for 2 h has essential no effect on its XRD pattern. 5. SUMMARY We have reviewed here the various routes that can be used tO prepare an extensive family of OMS and their precursors, OL. The syntl~c methods include the reflux, hydrothermaL precipitation, calcination, ion-exchange, isomorphous substitution, and sol-gel techniques. The materials compri~ OMS-1, OMS-2, and OL-1. The different synthetic methods have been compared, the important preparation parameters and reaction conditions have been identified. Various characterization techniques have been used to study the structure, comlx~sition,
196 morphology, and ~ stability of these materials. Both tunnel ( i o n - e x ~ e ) and framework substituted (dopants in solution precursors) materials have been reported. We have shown quite different physical and chemical properties of these matenals and how they are related to the resultant strucaae and to particular synthetic methods used to prepare such materials. REFERENCES
1. Lobo, R.F., Pan, M; Chan, I., Li, H.X.; Medmd, R.C., Zones, S.I.; Crozier, P.K, Davis, M.E. Science, 1993, 262, 1543-1546. 2. (a) Kresge, C.T.; Leonowicz, ME.; Roth, W.J., Vartuli, J.C., Beck, J.S. Nature, 1992, 359, 710712. (b) Inagaki, S.; Fukushima, Y.; Kuroda, IC J. Chem. Soc. Chem. Comm. 1993, 680. 3. Soghomonian, V.; Chen, Q., Haushalter, R.C.; Zubieta, J. Angew. Chem. Int. Ed Engl., 1993, 32, 610~11. 4. Tanev, P.T., Chibwe, M.; Pinnavaia, T.J. Nature, 1994, 368, 321-323. 5. Shen, Y.-F.; Zerger, I~P.; [kGuznum, R.N.; Suib, S.L.; McCurdy, L.; Potter, D.I.; O'Young, C.-L. Science, 1993, 260, 511-515. 6. O'Young, C.-L. in Expanded Clays and Other Microporous Solids; Occeili, M.L., Robson, H., Eds. Vol. II 333-340, Van Nostrand Reinhold, NY 1992. 7. DeGuzman, R.N., Shen, Y.-F., Neth, E.J., Suib, S.L., O'Ytmng, C.-L., ~ , S., Newsam, J. M., Chem. Mater., 1994, 6_,815-821. 8. Dumt, N., Suib, S.L., O~roung, C.-L. J. Chem. Soc. Chem. Comm. 1995, 1367-1368. 9. Shen, Y.-F., Suib, S.L., O~Young,C.-L., J. Amer. Chent Soc., 1994, 116, 11020-11029. 10. Ching, S.; Landfigan, J.K, Jorgensen, M.L., Duan, N., Suib, S.L.; O'Young, C.-L. Chem. Mater. 1995, 7, 1604-1606. 11. Yin. Y.-G., Xu, W.-Q., DeGuzma~ R.N., Shen, Y.-F., Suib, S.L., O'Young, C.-L., in Zeolites and Related Microporous Materials: State of the Art 1994, J. Weitkamp et al. Eds. pp. 1671-1676, Elsevier, 1994. 12. DeCnmnan, R.N., Shen, Y.-F., Shaw, B.I~, Suib, S.L.; O'Yom~ C.-L. Chem. Mater., 1993, 5, 1395-1403. 13. Shen, Y.-F.; Suib, S.L.; O'Young, C.-L. submitted for publication. 14. Golden, D.C., Chen, C.C., Dixon, J.B. Science, 1986, 231,717-719. 15. Tamada, O., Ymnan~to, N. Minerlt~c~ J., 1986, ~ 130-140.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
197
S y n t h e s e s a n d c r y s t a l s t r u c t u r e s of t w o " o r g a n o z e o l i t e s " K. Maeda, J. Akimoto, Y. Kiyozumi, and F. Mizukami National Institute of Materials and Chemical Research, Tsukuba, Ibaraki 305, Japan
Synthesis conditions of two isomeric aluminum methylphosphonates were examined. A1MepO-~t crystallized from a well-dispersed mixture of pseudo-boehmite, methylphosphonic acid and water on hydrothermal reaction. Neutral or acidic organic additives also favored formation of A1MepO-[~ with crystal size enlargement in most case. Static mixing followed by aging or use ofglycolic solvent instead of water caused to form AlMepO-a. Single crystal X-ray structural analysis of the two products revealed that both compounds have unidimensional channels lined with methyl groups. Also two new phases, designated A1MepO-~ and -5, were found. 1. I N T R O D U C T I O N Much attention has been paid to metal organophosphonate with a lamellar s t r u c t u r e as i n t e r c a l a t i o n hosts or d e s i g n e d l a y e r e d m a t e r i a l s [1]. Organophosphonic acid (RPO3H2) have an organic group (R) covalently bonded with the phosphorus center and the structure of metal organophosphonate generally has similarities with that of related phosphate [2,3]. However, structures other t h a n layered type were rare so far. Aluminum [4] and copper [5] methylphosphonates, and zinc aminoethylphosphonate [6] reported recently possess three-dimensional neutral frameworks and unprecedented organically lined tunnel structures. Such three-dimensional frameworks will provide possibilities for designed channel structures. The copper and zinc compounds have so small space surrounded by organic moieties that even nitrogen molecules perhaps cannot intrude. On the other hand, both of the isomeric aluminum methylphosphonates, A1MepO-a [7] and A1MepO-[~ [4,8], reported by us have as _large channels as can adsorb 2,2-dimethylpropane with a kinetic diameter of 6.2/~. They can be called the first "organozeolites" with molecular sieving properties. Their frameworks are different from existing aluminum phosphate molecular sieves [9] because P/A1 ratio should be 1.5 to build neutral framework and each phosphorus center should be connected to only three aluminum centers via oxygen atoms. We report here the synthesis condition and comparison of these two isomeric structures.
198 2. EXPERIMENTAL 2.1. S y n t h e s i s a n d c h a r a c t e r i z a t i o n Aluminum source was pseudo-boehmite powder (PURAL SCF, Condea Chemie, 74.4 wt.% A1203, 25.6 wt.% water). Methylphosphonic acid was obtained from Aldrich. Other organic reagents were obtained from Tokyo Kasei and used without further purification. Fundamental synthesis procedures were as follows: ten mmol of pseudo-boehmite powder and 15 mmol of methylphosphonic acid were dispersed in 400 mmol of water. The mixture (1.0A1 : 1.5P : 40H20) was stirred at ambient temperature for 1 h. The suspension was hydrothermally treated using an autoclave with a teflon sleeve at 160 ~ for 48 h in an thermostated oven under an autogenous pressure. The solid product was filtered, washed with water, and air-dried. In some runs, 5 mmol of an organic additive listed in Table 1 were added to the starting mixture or 10 g of organic solvents listed in Table 2 were used instead of water. Static mixing, namely gentle pouring of water onto boehmite covered with methylphosphonic acid followed by static aging of the mixture, was also examined instead of stirring in the mixing procedure. X-ray powder diffraction analyses (XRD) were performed with a MAC Science MXP18 diffractometer. Scanning electron microscopy (SEM) images were taken on a Hitachi S-800 microscope. 2.2. X-ray c r y s t a l l o g r a p h y Large crystals suitable for single crystal X-ray diffraction study were obtained from a different composition of mixture (1.0A1 : 1.0P : 40H20, reacted at 220 ~ for 48 h) for A1MepO-a and by addition of dioxane (1.0A1 : 1.5P : 40H20 : 0.5dioxane) for A1MepO-f3. X-ray diffraction data were taken on Rigaku AFC-4 diffractometer for A1MepO-a and Rigaku AFC-7 for A1MepO-f3. Crystallographic data for A1MepO-a: space group, trigonal P31c; a=13.9949(13), c=8.5311(16), Z=6; for A1MepO-~: space group, trigonal R3c; a=24.650(2), c=25.299(5), Z=18. Refinements were based on F2; the final Rw(F2) were 0.1081 (for 1795 reflections, 104 parameters) for A1MepO-a and 0.2115 (for 2514 reflections, 312 parameters) for A1MepO-f~.
3. R E S U L T S AND DISCUSSION
3.1. Synthesis conditions Figure 1 shows XRD of samples prepared with no additive (la) and aqueous ammonia (lb). With no additive the product gives XRD pattern with an intense reflection at d=12.30 corresponding to A1MepO-~. A1MepO-~ was obtained also at 130 ~ whereas a different compound, designated A1MepO--8, giving the strongest reflection at d=9.59 became the major product above 200 ~ Addition of aqueous ammonia caused to form another product, designated AlMepO-~, of non-porous layered structure with the composition AI(OH)(O3PCH3)'H20 [10]. Products obtained with various high-boiling organic additives were listed in
199 Table 1. Most of carboxylic acids, alcohols and ethers, namely acidic and neutral additives, gave A1MepO-[3 as the main product. Glycolic acid and oxalic acid did not give A1MepO-[3 probably owing to their strong chelation of aluminum. Basic additives like q u a t e r n a r y ) 9 9 b ammonium hydroxide, aqueous ammonia always gave A1MepO-~. Quaternary ammonium halide had no effect on product. These results revealed that quaternary ammonium 5 ' io ' a'o ' 4'0 hydroxide does not work as 20 structure-directing agent like in A1PO4 system [11] but works simply as base. Figure 1 XRD of A1MepO-[3 and -~ prepared with Hydrophobic interaction be- no additive (a), and aqueous ammonia (b), respectween methyl groups must tively. assist formation of the chan- 9 : A1MepO-[3, A : A1MepO-~ nel structure of A1MepO-[3. When the starting materials were mixed statically and left standing before the hydrothermal reaction, products changed depending on standing time. When the starting mixture was hydrothermally treated immediately after the water addition, the products contained mainly A1MepO-[5 (Figure 2a). On standing of the starting mixtures for 24 or 48 h A1MepO-a was mainly formed with small amount of A1MepO-[3 ,-~, -5 (Figure 2b and 2c). The maximum A1MepO-a content of the
I
9
9
.[
9
qp
.
9
9
9
Table 1 A1MepO products obtained with various organic additives Additive
Product
no additive [3>>~ AcOH [3>>~ AcOH (1.0) ~>~ PhCOOH (5 CH3(CH2)loCOOH ~ HOCH2COOH ~,Uk (COOH)2 (0.25) Am HOOC(CH2)4COOH* ~
Additive
Product
1-BuOH [3 2-BuOH [3>>~ t-BuOH [3>~ Ethylene glycol [3>~ 1,4-HO(CH2)4OH [3>~ Dioxane [3 Dioxane (1.5) [3 18-crown-6 [3>Uk
Additive
Product
NH3 NH3 (1.5)
[N(CH3)4]O H [N(C2Hs)4]OH [N(C3H7)4]OH [N(C4H9)4]O H [N(C4H9)4]Br
Additive/A1 = 0.5 unless ratio is given in parenthesis, *Additive/A1 = 0.25 Uk: Unknown phases, Am: Amorphous,
%>>Uk
[3
200 Table 2 Products from nonaqueous solvents. Solvent
Product
Ethanol a,~ Ethylene glycol a>>~ Diethylene glycol a,~ Tetraethylene glycol 1,2-Propanediol a>~ 1,3-Propanediol a,~ 1,4-Butanediol Glycerol a>>~ Dioxane Am>~ Water Am: Amorphous
o 9
J
9 li
1
9? 9
9
..
9
,"
t--
Lt
c-
purest sample so far obtained • 9 9 is c a . 9 1 % according to 27A1 9 9A 9 A 9 9 9 A~A 9 9 J MAS-NMR. Pure and large crystals of A1MepO-a were obtained from starting mixture ,, . /~ 1 .. , a) of the composition 1.0AI : 1.0P : 40H20 reacted at 220 ~ for 1'o ' go ' 3b ' 4'o S 48 h (Figure 2d) as described 2(1 above. Careful s e p a r a t i o n from boehmite-derived mass, Figure 2 XRD of products obtained with however, was necessary and different aging time in static mixing. a) 0 h, b) 24 h, c) 48h, d) single crystals the yield was very low. Nonaqueous organic solvents prepared from composition 1.0A1 : 1.0P : 40H20 have been used to produce at 220 ~ novel materials and large crys9 : A1MepO--a, 9 : A1MepO-~, • : AIMepO--5, tals in zeolite-related material A : A1MepO-~ synthesis [12,13]. The effect was claimed to be owing to reducing amount of water in the reaction media. In our system, alcohol was effective as solvent to obtain microporous products; non-hydric dioxane gave small amount of crystalline product. Many alcohols listed on Table 2 tended to give product containing A1MepO-a in spite of mixing by stirring, although static mixing is necessary for formation of A1MepO--a in the case of water solvent. Especially, ethylene glycol and glycerol was most suitable to obtain A1MepO-a. With no additive the dimension of A1MepO-~ needle crystals ranges c a . 30-300 ~tm in length and less than 10 ~tm in width (Figure 3a). Sometimes small amount of AlMepO-~ was observed as plate crystals together with A1MepO-~. A1MepO-~ synthesized with aqueous ammonia was aggregates of plate crystals (Figure 3c). Instead of no templating ability of the acidic and neutral additives, most of them stimulate growth to give larger crystals; among them dioxane was most effective to
J
201
a)
V. I l l l l l l
b)
Him
V. ! ! [1111
el)
Figure 3 SEM Image of A1MepO products a) A1MepO-[3 with no additive, b) A1MepO-[3 with dioxane, c) A1MepO-~ with aqueous ammonia, d) A1MepO-a by static mixing.
202 give approximately ten times larger crystals than no additive (Figure 3b). Elemental analysis revealed that a considerable amount of dioxane remains in the crystals even after thorough washing with water, although a trace amount remain in products from other additives. Good fit of dioxane molecules into channels probably encourages crystal growth along the channels, i.e. in the direction of the needle. As can be seen in some SEM images the needle crystals were often observed as radial aggregates typically in spherical or conical shape or as needles twinned on the side. This indicates that nuclear growth starts from small boehmite particles dispersed in water followed by collapse of the aggregates into separate needle crystals. Crystals of AlMepO--a synthesized by static mixing were also long needles similar to A1Mel~O-~ of 50-1000 ~m in length (Figure 3d). Optimum synthesis conditions of A1MepO-a suggest that less dispersed boehmite in reaction media favors formation of this phase. Anyhow, further study is necessary to obtain full understanding of the reaction mechanism. 3.2. C r y s t a l s t r u c t u r e s Both structures have the same framework composition A12(CH3PO3)3 and contain both tetrahedral (/kiTh) and octahedral aluminum (A1oh) in the ratio of 3 : 1 as also confirmed by 27A1 MAS-NMR. The frameworks are composed of vertex-shared [A1ThO4], [A1ohO6] and [CH3PO3] polyhedra. The arrangement of Aloh is similar between the two frameworks. Each Aloh is surrounded by eight nearest A1Oh; two are located almost along the c-axis and the other are along the channel walls. The connectivity among A1Ohis different between the isomers as shown in Figure 4. In AlMepO-a [7] three-fold rotation axes parallel to the c-axis run through the positions Where every A1Oh (All in Figure 4a) locates. Therefore, there are only two independent phosphorus sites (P1 and P2). The connectivity along the c-axis is
I a
I ~ b
Figure 4 A1-P linkage of A1MepO-a and-[5. a) left, viewed along [110], b) right, viewed along [120] white circle: A1oh, black circle: methyl group
a
C
203 9
9
~l
eQ.
.~
.\
Io
\X'"
T ,
9 ;
9
Figure 5 Stereoplots of AlMepO-a (top) and-13 (bottom) viewed along [001]. whitecircle: A1oh, black circle: methyl group based on the stacking of 6343 polyhedra sharing vertex A1Oh(Figure 4a). Along the channel wall two A1Ohare connected by single linkage. In A1MepO-~ [8], three-fold screw axes parallel to the c-axis run beside the positions where every Aloh (All in Figure 4b) locates. Each A1oh is connected with two AlOh almost along the c-axis by linearly fused triple four-rings in which the two extreme rings are on the same side of the central four-ring (Figure 4b). Each AlOh is connected with further two Aloh among the remaining six neighbors by similar triple four-rings in which the two extreme rings are on the opposite sides of the central ring. Figure 5 showed stereo drawing of the frameworks along the c-axes. Unidimensional straight channels are running along the c-axes. The oxide frameworks surrounding the main channels contain triangular 18-ring as large as VPI-5 [14], a representative large pore aluminophosphate. So far reported phosphonates [5,6] and phosphites [15,16] with channel structures lined with organic groups or hydrogen atoms connected to phosphorus centers contained 12-rings at largest. The channels of both compounds are lined with methyl groups. In A1MepO-a and -~, large channels composed of 18rings allow to leave still large space where the inner wall are covered with methyl groups.~ A cross section of a channel of A1MepO-a looks triangle, a side of which is c a . 7.0 A. In A1MepO-~ a channel section is of similar size as A1MepO-a and looks
204 rather rounded because the channel wall are more rugged and twisted along the triangular channel than A1MepO-a.
CONCLUSIONS Optimization of synthesis conditions including organic additive, reaction solvent, mixing and aging conditions enables selective synthesis of two structural isomers of aluminum methylphosphonate "organozeolites". Organic additives do not work as template like A1PO4 synthesis but affect crystal size. Channel structures lined with organic groups are confirmed by single crystal X-ray structural analysis.
REFERENCES
1. 2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16.
T.E. Mallouk and H. J. Lee, Chem. Edu., 67 (1990) 829. Y.P. Zhang and A. Clearfield, Inorg. Chem., 31 (1992) 2821. G. Cao, H.-G. Hong and T. E. Mallouk, Acc. Chem. Res., 25 (1992) 422. K. Maeda, Y. Kiyozumi, F. Mizukami, Angew. Chem. Int. Ed. Engl., 33 (1994) 2335. J. Le Bideau, C. Payen, P. Palvadeau, B. Bujoli, Inorg. Chem. 33 (1994) 4885. S. Drumel, P. Janvier, D. Deniaud, B. Bujoli, J. Chem. Soc., Chem. Commun., (1995) 1051. K. Maeda, J. Akimoto, Y. Kiyozumi, F. Mizukami, Angew. Chem. Int. Ed. Engl., 34 (1995) 2335. K. Maeda, J. Akimoto, Y. Kiyozumi, F. Mizukami, J. Chem. Soc., Chem. Commun., (1995) 1033. J.A. Martens and P. A. Jacobs, in Advanced Zeolite Science and Applications, eds. J. C. Jansen, M. StScker, H. G. Karge and J. Weitkamp, Elsevier, Amsterdam, 1994, p. 653-685. K. Maeda, to be published. E.M. Flanigen, B. M. Lok, R. L. Patton and S. T. Wilson, inNew Developments in Zeolite Science and Technology, eds. Y. Murakami, A. Iijima and J. W. Ward, Elsevier, Amsterdam, 1986, p. 103. Q. Huo, R. Xu, S. Li, Z. Ma, J. M. Thomas, R. H. Jones and A. M. Chippindale, J. Chem. Soc., Chem. Commun., (1992)875. A.F. Kuperman, S. Nadimi, S. Oliver, J. Garces, M. M. Olken and G. A. Ozin, Nature, 365 (1993) 239. M.E. Davis, C. Saldarriaga, C. Montes, J. Garces and C. Crowder, Nature, 331 (1988) 698. R.E. Morris, M. P. Attfield and A. K. Cheetham, Acta. Crystallogr. Sect. C, 50 (1994) 981. M. Sghyar, J. Durand, L. Cot and M. Rafig, Acta. Crystallogr. Sect. C, 47 (1991) 2515.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
205
ERS-8: a N e w Class of Microporous A l u m i n o s i l i c a t e s
Giovanni Perego, Roberto Millini, Carlo Perego, Angela Carati, Giannino Pazzuconi and Giuseppe Bellussi Eniricerche S.p.A., Via F. Maritano 26, 1-20097 San Donato Milanese (Italy)
The synthesis of micro-mesoporous aluminosilicates via gelation of a reaction mixture containing Si(OC2H5)4, AI(OC3H7)3, C2HsOH, H~O and alkali-free NR4-OH (R = C3H7, C41-I9, CsH m C8H~3) is described. X-ray amorphous mesoporous aluminosilicates (MSA) or microporous alominosilicates, characterized by a broad peak in the low angle region of XRD pattern (ERS-8), are obtained, depending on the NR4-OI-I/SiO2molar ratio and on the number of C atoms in the R groups. A structural model is proposed concerning the arrangement of the NR4§ cations within the gel, which accounts for the experimental data.
1. INTRODUCTION M41S constitutes a well known class of ordered mesoporous materials which is formed in hydrothermal conditions, starting from an aqueous solution containing silica and alumina sources together with CiH2i§ N§ cations (i > 7; usually 12 or 16) [ 1,2]. The same procedure can be used for preparing mesoporous materials containing oxides of V [3], Ti [4], Mn [5], W [6], Sb [6]. A mechanism of formation of M41S has been proposed, based on the templating effect of a liquid crystal structure formed in the reaction mixture by tetraalkylammonium cations, due to their surfactant properties [1,2]. For the MCM-41 derivative, Stucky et al. [7] suggested the initial formation of a lamellar structure of surfactant molecules interposed between sheets of silica oligomers, which transforms into the hexagonal mesophase as polymerization of silica proceeds. After the discovery of M41S-type compounds many attempts have been made to synthesize new ordered porous materials. We claimed the possibility to synthesize mesoporous X-ray amorphous aluminosilicates (MSA) with a narrow pore size distribution [8,9]. The procedure initially adopted was based on the gelation, eventually followed by a hydrothermal treatment at 180~ of an alkali-free mixture of silica and alumina sources in the presence of (C3H7)4N-OH. Successively, an easier and more reproducible procedure was adopted, based on
205 refluxing a hydroalcoholic solution of the silica and alumina sources, in the presence of (C3H7)4N-OH as gelating agent [10]. Though it is known that the textural properties of amorphous aluminosilicates can be controlled by gel formation in acidic [11] or slightly basic media [12], the synthesis of MSA is performed under strongly basic conditions in order to stabilize tetrahedral A1 [13]. This gives MSA interesting properties in acid-catalyzed reactions [8-10]. Starting from the formation mechanism postulated for MSA, we investigated the synthesis parameters which in principle could modify the arrangement of NR4§ cations in the gel, arriving at the discovery of a new class of materials (named ERS-8). The paper deals with the synthesis and characterization of ERS-8's compared to MSA's. 2. EXPERIMENTAL The materials investigated were prepared using Si(OC2H5)4 (Dynasil-A, Nobel), AI(i-OC3H7) 3 (Fluka) or AI(8-OC4H9) 3 (Fluka), aqueous alkali-free NR4-OH (R - C2H5, C3H7, C4H9, C5Hll, C6H13), ethanol and distilled water. The molar ratios EtOH/SiO 2 = 8, H20/SiO 2 = 8, SiO2/A1203 - 50 were kept constant for all the runs, varying the molar ratio NR4+/SiO2 in the range 0.03 to 0.40. In a typical preparation, AI(/-OCsH7) 3 is dissolved in aqueous NR4-OH at 60~ to which an ethanolic solution of Si(OC2H5)4 is added under vigorous stirring. When using (C6H13)4N-OH (40% wt in water), this is diluted with EtOH and then with the required amount of water before being mixed with a solution of Si(OC2Hs) 4 and AI(s-OC4H9) 3. In both procedures the initial clear solution becomes a viscous gel in a few minutes. After about 15 hours aging at room temperature, the gel is dried at lOO~ and calcined at 550~ during 8 hours in air flow. The solid products were characterized by: - X-ray powder diffraction (XRD) on a computer controlled Philips diffractometer using CuKa radiation (~ = 1.54178 A). In the angular range 1< 2(} < 10 ~ the data were collected stepwise with 1/6~ receiving slit set. The position and breadth of the Bragg peak were accurately determined by means of the FIT routine contained in the software package DIFFRAC (from Siemens), assuming a Split-Pearson VII function for the peak profile. - Thermogravimetric analysis (TGA), with a Mettler TG50 thermobalance controlled by a Mettler TC 3000 microprocessor, running in the range 25 - 900~ heating rate 10~ and 300 ml/min air flow. - Nitrogen physisorption on a computer controlled Fisons Sorptomatic 1990 system. The calcined samples were degassed under high vacuum (~ 10.5 torr) at 300~ for 4 hours. The data were analyzed with the Horvath-Kawazoe method [14]. 3. RESULTS AND
DISCUSSION
As previously reported [8-10], X-ray amorphous aluminosilicates (MSA), characterized by a narrow pore size distribution, can be obtained by using
207 (C3H7)4N-OH as a gelling agent. The same type of materials can be obtained by using other NR4-OH compounds (R = C4H9, C5Hll, Cell13), provided the synthesis is carried out with low NR4-OH/SiO 2 molar ratio [8,10,15]. When performing gelation with higher NR4-OH/SiO 2 molar ratios, we obtained materials different from MSA, characterized by the presence of a peak in the low angle region of the XRD pattern and by a very narrow pore size distribution, with pore radius constantly lower than 20 A [15]. Table 1 Characteristics of the synthesized materials. Sample a NR4-OH/SiO 2 Vol. fraction (%)b
Phase type
d (A) ~
dried d
calcined e
C3(1)
molar ratio 0.403
NR4§ 75
SiO 2 25
ERS-8
19
56
C3(2)
0.253
65
35
ERS-8
20
54
C3(3)
0.197
60
40
ERS-8
18
51
C3(4)
0.153
53
47
ERS-8
19
47
C3(5)
0.113
45
55
MSA
C3(6)
0.105
42
58
MSA
C3(7)
0.093
40
60
MSA
-
C6(1)
0.256
78
22
ERS-8
25
4O
C6(2)
0.108
60
40
ERS-8
24
32
C6(3)
0.082
53
47
ERS-8
26
31
C6(4)
0.068
48
52
ERS-8
25
32
C6(5)
0.062
45
55
MSA
C6(6)
0.047
41
59
MSA
C6(7) C6(8)
0.038 0.034
35 33
65 67
MSA MSA
C6(9)
0.032
30
70
MSA
C6(10) 0.030 28 72 MSA (a) The labels C3(X) and C6(X) stand for materials prepared with R = C 3 H 7 and C6H13, respectively. (b) Referred to dry gels; assumed mass densities of 0.9 and 2.0 g/cm 3 for NR4+ and SiO2, respectively. (c) Bragg distance in XRD pattern. (d) At 100~ in air. (e) At 550~ in air during 8 hours. Starting from these results, a systematic varying both the NR4-OH/SiO 2 ratio and the the other synthesis parameters constant (see volume fractions of SiO 2 and organic matter
investigation was carried out by chain length of R groups, keeping Experimental). By referring to the in the dried materials (derived by
208 assuming for both components reasonable values of mass density, see Table 1), it appears very clearly that a threshold exists around 50% volume fraction of NR4§ Below this threshold, MSA is formed while above this ERS-8 is formed, independent on NR4§ used in the synthesis (Figure 1) In a previous paper, a detailed characterization was given for MSA prepared with (C3H7)4N-OH [9]. To better describe the properties of ERS-8's compared to those of MSA's, attention will be focused on the materials prepared with R = C3H 7 and Cell13 (Table 1) considering that the same conclusions are valid for materials obtained with R = C4H9 and CsHlr The only exception is R = C2H5 which gives MSA over the whole range examined. A peak is observed in the XRD pattern of as-synthesized, 100~ and calcined ERS-8's; however, the position of the peak varies significantly as a function of the thermal history of the sample (Figure 2). i
9
i ERS-8
MSA
D
!i5
I,m i
3
A
l'o 2~ 3'0 4~ 50 6'0 7o ~'o ~, ioo
0
NR4 Vol.fraction(%)
Figure 1. Relationship between the NR4+ volume fraction in wholly dried precursor and the type of material obtained ~ I S A , @ERS-8).
4
2
6
8
2-Th eta [o]
10
Figure 2. Low angle region of XRD patterns for as-synthesized (A), dried at 100~ (B) and calcined at 550~ (C) ERS-8 (sample C6(2)), compared to that of MSA (D) (sample C6(7)). 40
N
"
i /
\
:x
/
i
"|
""
l '~-
34
~:ir-dried
.~
32
-o
263028 24
-
-
-
i
-
-
i
.
.
.
.
f
.
-
-
i
"
-
Figure 3. TG ( - - ) and DTG (.... ) curves of dried C6(2) sample.
as-synthesized gel
38
36
22
gel
~""B'"r"~
1()0
-
2()0
3()0
Temp. (~
400
5(}0
600
Figure 4. Variation of d as a function of calcination temperature, for ERS-8 sample C6(2).
209 The FWHM (3 - 4 ~ 20) of the peak is quite large and certainly indicative of very low structural order; however, it is significantly lower than the FWHM (8 10 ~ 20) of the peak (observed in both MSA's and ERS-8's) at ca. 23 ~ 20, due to the Si(A1)/Si(A1) pair correlation. Whether the low angle peak has to be considered a Bragg peak may be matter of discussion. In any case, it seemed reasonable to consider the related Bragg distance, d. The trace of the TGA curve, shown in Figure 3 (the same features were observed in all the dried gels), is characterized by several steps of weight loss, which are interpreted as in the following. Below 150~ residual H~O and C2HsOH are lost, while the organic matter is eliminated in two well defined steps. The first one (at ca. 270~ corresponds to the elimination of NR4-OH molecules simply "embedded" in the aluminosilicate matrix; in the second one (at ca. 350~ the elimination of NR4+ acting as counterions to the tetrahedrally coordinated A1 ions occurs. As a matter of fact, both in MSA's and in ERS-8's, the moles of NR4§ lost at higher temperature nearly correspond to the total moles of AI present in the material. The slight weight loss observed at T > 450~ probably corresponds to the combustion of some coke formed during the TG analysis and/or to the elimination of H20 deriving from condensation of surface silanol groups. Portions of C6(2) dried gel were treated in the T G furnace at the temperatures indicated in Figure 3. The X R D peak is observed for all the samples and the related Bragg distance, d, varies as a function of the treatment tempoerature (Figure 4). The value of d decreases from ca. 38 A (wet gel) to ca. 24 A in the totally dried sample (150~ and increases up to ca. 32 ik after calcination at 550~ It is worthy to note that, for dried samples, the value of d is practically independent of the NR4-OI-I/SiO 2 molar ratio, but depends on the number of C atoms of the R groups (Table 1).
9 o
9
o
9
MSA
9
o 0"6
~
0.4
L/.~':":"...... ~RS~
~
.eo.eO-eo''
9
9
9
ERS-g
,,P o
04
o g
o o
o
9
MSA
mO~ 0 0 ~0.2 o~d~
. . . . . . . .
i i0
.
.
.
Pore radius
. (~)
.
. 100
.
.
. . . . . . .
. 1000
o~
| 10
,j 100 Pore radius
. . . . . . . . 1000
(,~)
Figure 5. Cumulative pore volume of MSA Figure 6. Cumulative pore volume of MSA (sample C3(5)) and ERS-8 (sample C3(3)) (sample C6(7)) and ERS-8 (sample C6(2)) synthesized with (C3H7)4N-OH. synthesized with (CsH13)4N-OH. The pore size distribution is narrow in both materials. However, while in MSA there is a predominance of mesopores, in ERS-8 only micropores (r in the range 3
210
10/k) are present, independent on NR4 § used (Figures 5 and 6). Both MSA's and ERS-8 are characterized by specific surface area in the range 700 - 1000 m~/g. Pore volume of M S A is ranging from 0.5 to 0.7 cmS/g (C3 series) and from 0.4 to 0.5 cm3/g (C6 series);for ERS-8, values of 0.3 - 0.4 cm3/g (C3 series) and 0.4 - 0.5 cmS/g (C6 series) are measured. The following model is given, which reasonably accounts for the experimental data. In the gelation step, the formation of clusters of NR4 § cations is postulated. The picture shown in Figure 7 represents a possible structure for these clusters, where the alkyl chains in liquid-like conformation are arranged parallel to one another; the O H anions solvated by ethanol and water molecules are placed on the border of the alkyl chains assembly. In MSA-forming mixtures, the growth of these clusters is limited because of the excess of silica (volume fraction exceeding that of NR4 § see Table 1) which tends to form a three-dimensional aluminosilicate structure all around them (Figure 8a). As a consequence, the ethanol- and water-containing NR4 § domains become the pore precursors of M S A (Figure 8b) and their dimensions control the pore size of the material. In an ERS-8-forming mixture, due to the excess of NR4 § component with respect to silica(see Table 1), the NR4 § clusters are expected to grow much more in the directions perpendicular to that of the elongation of the alkyl chains. Practically, the formation of monolayers of NR4 § solvated by ethanol and water molecules, is admitted, on the surface of which aluminosilicate sheets grow. According to this hypothesis, the ERS-8 precursor has to be considered essentially as a layered-type material. The layers so formed should be embedded in ethanol and water (which constitute about 90% of the total volume of the gel) with occasional, if any, layers stacking. Therefore the d value of 38 A would represent the average distance between the aluminosilicate sheets grown on the two surfaces of each NR4 + layer (Figure 8c). It is interesting to note that the formation of a layered-type intermediate has been proposed also for M C M - 4 1 [7]. After drying, the structure should collapse with a resulting packing of the layers roughly parallel to one another. The decrease of d value for the dried gels is well accounted for by the removal of most of ethanol and water molecules from the interlayer region (Figure 8d). Consistently with the different length of the alkyl chains of NR4 + cations, the d values observed for C3 samples (18 - 20/k) are lower than those observed for C6 samples (24 - 26/k, see Table 1). However, according the poor order of the structure, only occasional correlation exists among the layers along the direction parallel to the stacking direction (no correlation at all in the other directions). As the organic matter is removed during calcination, the two aluminosilicate sheets grown on each NR4 § layer will condense forming double sheets; these constitute the building blocks which form a three-dimensional structure (through inter-sheet condensation of silanol groups), maintaining the plane of the sheets roughly parallel to each other. Due to the likely difference in the dimensions (mainly length and width) of the sheets, a regular assembly cannot occur and pores are inevitably formed. In Figure 8e a simplified, very schematic picture of the 3D structure proposed for ERS-8 is shown. According to this model, pore -
211
dimensions in the direction perpendicular to the plane of the sheet (arrows in Figure 8e) is controlled by the double-sheet thickness, which is expected to be much more regular than length and width (for this reason, a broad distribution of pore dimensions is expected along the directions parallel to the sheet plane). Since the average thickness of a single sheet is estimated to be around 5 A (by considering the d value together with the volume fractions of
- Nl~luster
MSA
ERS4~
3s~ a
I dryingand ! calcination
~ dr~.g
d
Figure 7.
Proposed structure for a
solvated (C2Hs-OH + H20)(C6H13)4 N+
/calcination
Figure 8. Schematic model proposed for pores formation in MSA and ERS-8
clusters (number of molecules arbitrary). NR4§ and S i O 2 ) , w e should expect pore dimensions of ca. 10/k (one double sheet), ca. 20/~ (two double sheets), etc. The curves of Figures 5 and 6 really agree with the presence of pores of ca. 10 and ca. 20/~ in ERS-8's. Inter-sheet distances can be identified within the structure (arrows in Figure 8e), not correlated to each other, which account for the broad Bragg peak observed in calcined ERS-8's. These distances correspond to multiples of the average thickness of the double sheet. The d values observed for calcined ERS-8 (Table 1), agree with an average of 3-4 double sheets (C6 series) and 4-5 double sheets (C3 series). Because the pore size distribution is practically identical for the two materials, the larger spacing observed for C3 series may be accounted for by a more dense
212 packing of the sheets. The lower value of total pore volume observed for ERS-8 in C3 series, relative to that in C6 series, agrees with the above hypothesis. 4. CONCLUSIONS Gelling a solution containing silica and alumina sources with an alkali-free tetraalkylammonium hydroxide (NR4-OH, R = C3H 7, C4H 9, CsH n, C8H13) leads to the formation of mesoporous (MSA) or microporous (ERS-8) aluminosilicates. In particular, the formation of ERS-8 occurs when the volume fraction of NR4 § exceeds that of silica-altunina, independent on the length of R alkyl chain. ERS-8's represent a new class of aluminosilicates characterized by a narrow pore size distribution in the range of micropores. Due to their acidic properties, these materials are suitable for applications in acid-catalyzed reactions. REFERENCES 8
Q
~
*
5. 6. 0
0
1
10. 11. 12. 13. 14. 15.
C.T. Kresge, M.E. Leonowicz, W.J. Roth, J.C. Vartuli and J.S. Beck, Nature 359 (1992) 710. J.S. Beck, J.C. Vartuli, W.J. Roth, M.E. Leonowicz, C.T. Kresge, K.D. Schmitt, C.T.-W. Chu, D.H. Olson, E.W. Sheppard, S.B. McCullen, J.B. Higgins and J.L. Schlenker, J. Am. Chem. Soc. 114 (1992) 10834. I~M. Reddy, I. Moudrakovski and A. Sayari, J. Chem. Soc., Chem. Commun., 1059 (1994) P.T. Tanev, M. Chibwe and T.J. Pinnavaia, T.J., Nature 368 (1994) 321. D. Zhao and D. Goldfarb, J. Chem. Soc., Chem. Commun., 875 (1995) Q. Huo, D.I. Margolese, U. Ciesla, P. Feng, T.E. Gier, P. Sieger, R., Leon, P.M. Petroff, F. Schuth and G.D. Stucky, Nature, 368 (1994) 317. A. Monnier, F. Schuth, Q. Huo, D. Kumar, D. Margolese, R.S. Maxwell, G.D. Stucky, M. Krishnamurty, P. Petroff, A. Firouzi, M. Janicke and B.F. Chmelka, Science 261 (1993) 1299. G. Bellussi, M.G. Clerici, A. Carati and F. Cavani, US Patent No. 5 049 536 (1991). G. Bellussi, C. Perego, A. Carati, S. Peratello, E. Previde Massara and G. Perego, Stud. Surf. Sci. Catal. 84 (1994) 85. C. Perego, S. Peratello and R. Millini Eur.Patent No. 659,478 A1 (22.12.1993) T. Pecoraro, U.S. Patent No. 4,988,659 (1991). M.R. Manton and J.C. Davidtz, J. Catal. 60 (1979) 156. J. Livage, Stud. Surf. Sci. Catal. 85 (1994) 1. G. Horvath and I~ Kawazoe, J. Chem. Eng. Jpn. 16 (1983) 470. G. Pazzuconi, G. Bassi, C. Perego, G. Bellussi, R. Millini and G. Perego, It. Patent No. 94A001399 (1994).
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
213
S y n t h e s i s a n d c h a r a c t e r i z a t i o n of l e v y n e t y p e zeolite o b t a i n e d f r o m gels w i t h different SIO2/A1203 ratios C. V. Tuoto a, J. B. Nagyb and A. Nastro a aDepartment of Chemical Engineering and Materials, University of Calabria, Arcavacata di Rende, 87030 Rende (CS), Italy bUnit~ de R.M.N., University of Namur, Rue de Bruxelles 61, B-5000 Namur, Belgium. Levyne type zeolites have been successfully synthesized from gels 4.5Na206MeQI-xAI203-30SiO2-500H20 with 0.6_<x_<3, at 150~176 The 29Si spectra show unambiguously the presence of two different crystallographic sites in the structure. The combined 13C-NMR and TA data allowed one to interpret the nature of two different types ofMeQ + ions in the levyne channels. 1. INTRODUCTION The structure of the levynite, a natural zeolite discovered in 1825 [1] can be described by a sequence of single six member rings [2]. The unit cell has a trigonal symmetry and contains 54 tetrahedral sites [36 T1 sites and 18 T2 sites]. The chemical composition of the levynite is Ca3(Al18Si36Olo8)50H20 and the diameter of the pores is 4.8 x 3.6A [2]. Its use as a molecular sieve and as a catalyst for the transformation of methanol to low molecular weight olefins has been recently demonstrated [3]. Although the levynite was one of the first discovered zeolite, its first synthesis was only reported in 1969, the zeolite ZK-20 was obtained from an aluminosilicate gel containing DABCO (1-Methyl 1-Azonia 4-azabyciclo [2,2,2] Octane) [4]. Later the synthesis of similar structures were reported such as Nu-3 [5], LZ-132 [6] and LZ-133 [7], b a s e d on t h e use of m e t h y l q u i n u c l i d i n e (1Methylazabicyclo[2,2,2]octane). The structure of LZ-133, not yet resolved, was claimed as being analogous to the levynite structure, although the X-ray pattern is quite different from that of levynite [7]. Zeolite ZSM-45 also of levynite structure was obtained in presence of 2-hydroxyalkyltrialkylammonium chloride [8]. It has to be noted that synthetic levyne-type zeolites all have a quite high Si/A1 ratio, because they were synthesized in presence of organic molecules. Quite recently, different hetero-atoms have also been introduced in the levyne structure [9,10]. Finally, levyne was also successfully obtained in fluorine containing media [11]. As the synthesis of levyne type zeolites is essentially described in the patent literature, it is interesting to explore the field of crystallization, the influence of the SiO2/Al203 ratio in particular [12,13]. In the present work are reported the results on the synthesis and on the characterization of levyne-type zeolite obtained from sodium aluminosilicate gels
214 containing methylquinuclidine iodide (MeQI) as organic compound and a variable SiO2/Al203 ratio. 2. E X P E R I M E N T A L
As the amount of sodium and methylquinuclidine iodide (MeQI) were previously optimised in the initial gels [12], in this study the relative amount of A1 was varied following=.. 4.5Na20-6MeQI-xA1203-30SiO2-500H20 with 0.6 < x< 3 -
-
n
The hydrogels were prepared by mixing the reagents in the following order: 30% aqueous solution of NaOH (pellets RPE, Carlo Erba), MeQI synthesized from quinuclidine (Aldrich) and iodomethane (Aldrich) following refs. 6 and 7, AI(OH)3 (dry gel, Pfaltz and Bauer), distilled water and SiO2 (fumed silica, Serva). The so obtained homogeneous gel mixtures were heated in sealed Teflon autoclaves (8 cm 3) at 150~ 170~ and 190~ in static conditions. A ~ r programmed periods of time, the autoclaves were quenched in cold water and the solid product filtered, washed with cold water and dried at 100~ for 12 hours. The gels, after 48 h of ageing at room temperature, were dried at 100~ for 24 h. The nature of the solid and the degree of crystallinity were determined by x-ray powder diffraction using a Philips PW 1730/10 diffractometer equipped with a PW 1050/70 vertical goniometer (CuKal). The reference sample for quantitative measurement were obtained from the final crystalline products treated with ultrasounds in order to separate the well crystallized material from the remaining amorphous gel. Thermal analyses (DSC, TG and DTG) of dried gels and of the crystalline products were made on a Netzsch STA 409 thermal analyzer scanning from 30~ to 800~ at a rate of 10~ under a 15ml/min air flow. The size and shape of the crystallites were measured by SEM on a JEOL JSMT 330A microscope. The chemical analysis was made by atomic absorption. The NMR spectra were recorded on either a Bruker MSL 400 or a Bruker CXP 200 Spectrometer. For 29Si (39.7 MHz) a 6.0~ts (0= ~/2) pulse was used with a repetition time of 6.0 s. For 13C (50.3 MHz), 5.0~ts (0=~/2) pulses, a single contact sequence with 5.0 ms contact time and a recycle time of 4.0s were used. For 27A1 (104.3 MHz), a 1.09s (0= ~/12) was used with a repetition time of 0.2s. 3. RESULTS AND DISCUSSION The crystallization field obtained at various temperatures and various SiO2/Al203 ratios is illustrated in Figure 1. Pure levynite crystals can be obtained at low temperature (150~ for SiO2/Al203 ratios up to 40, while at high temperature (190~ gels of only low SiO2/Al203 ratios can lead to pure levyne.
215
9
O
190 "
I
'
I
k
'
I
'
I
'
I
#"
~LEV+LZ133
O
d
~LEV+~
+Q
170
-
LEV
150 9
I
9
10
I
9
I
,
I
30
i
I
,
50
8iO2/A1203 ratio Fig. 1 Crystallization field of various crystalline phases obtained after 10 days of synthesis from 4.5Na20-6MeQI-xAI203-30SiO2-500H20. The absence of amorphous phase in the crystallization field underlines the importance of MeQ + in the formation of either LEV or LZ-133. Finally, at high SiO2/Al203 ratios, the more stable quartz phase also starts to form. Figure 2 shows the crystallization curves for systems with different x values at 150~ The induction rate (1/tind in h-l) and crystallization rate (R in % day "1) are determined from Figure 2. If log 1]tind and logR are plotted as a function of log x a linear correlation is obtained with a negative slope of-l.4. It seems thus that the amount of A1203 in the gel has a great negative influence on both the induction and crystallization rate.
100 80 60
D x=3.0 9 x=2.0 o x=l.5 9 x=l.2 A x=l.0
-r-0
~
40
~
20 0
A
0
5
10
x=0.8
15
Time, days Figure 2. Crystallization curves oflevyne as a function of x at T=150~ from gels 4.5Na20-6MeQI-xA1203-30SiO2-500H20.
216 Table 1. Physicochemical characterization of final crystalline levyne samples obtained at 150~ from the gels 4.5Na20-6MeQI-xA1203-30SiO2-500H20. Si/A1 gel 5
Si/Al H20/u.c 6.8
5.7
NaJu.c 2.5
Al/u.c MeQ+tot/u.c 7.2
4.8
MeQ+/u.c MeQ+/u.c DSC=480~ DSC=580~ ....
4.8
7.5
8.7
2.7
1.2
5.8
4.9
....
4.9
10.0
10.7
4.6
0.8
4.8
6.6
2.0
4.6
12.5 15.0
14.1 15.0
3.7 2.5
0.7 0.9
3.7 3.5
6.7 7.1
2.9 3.5
3.8 3.6
17.5
20.5
3.8
0.9
2.6
7.1
3.7
3.4
e
X=0.8
X O
X=l.O
x=1.2 x=1.5 e n
x=2.0
d O
X=3.0 0
200
400
600
800
TEMPERATURE, ~ Figure 3. DSC curves of crystalline levyne phases obtained at 150~ from gels 4.5Na20-6MeQI-xAI2 O3-30SIO2-500H20.
217 Table I shows the physicochemical characterization data of the final crystalline levyne samples. It is shown that the aluminium incorporation in the structure is quite effective, the Si/A1 ratios in the initial gels and in the final samples are quite close. The amount of Na + ions is quite low and decreases with decreasing A1/u.c. Oppositely, the total amount of MeQ + increases with decreasing Al/u.c. It is interesting to note that the thermal decomposition of MeQ + ions shows a low temperature peak at ca. 480~ and a high temperature peak at ca. 580~ (Figure 3). It can be interpreted, as it was previously shown for TPA + in ZSM-5 [15] or MeQ + in levyne of high Si]A1 ratio [16] , that the 480~ peak is due to the decomposition of MeQ + neutralizing SiO- defect groups, while the 580~ peak is due to the decomposition of MeQ + neutralizing (SiOA1-) negative charges. For the first two samples, with the highest A1 contents, only the high temperature peak is detected and the A1/u.c. is equal to (MeQ + M)/u.c. (Table 1). As the Al/u.c. is decreasing, the low temperature peak appears and its amount increases with decreasing Al/u.c. In these cases the sum of the amount of high temperature MeQ and the amount of M/u.c. is always higher than the Al/u.c. (Table 1), showing the presence of defect groups in the structure. The presence of these defect groups is confirmed by the high resolution solid state 29Si-NMR spectra of levyne samples. Figure 4 and Table 2 show the 29SiNMR results. The NMR line at-115 ppm can be tentatively assigned as stemming from Si(OA1)configurations ofT2 sites. The-108.5 ppm is then assigned to Si(1A1) configuration on T2 and to Si(0A1) of sites T1. The -103.2 and -97.3 lines are s u p p o s e d to s t e m , r e s p e c t i v e l y , from Si(2A1)T2+Si(1A1)T1 and Si(3A1)T2+Si(2A1)T1. In addition, a rather large contribution of the defect groups SiOM and SiOM2 (M=Na and/or H) can be found in lines -103.2 and -97.3 ppm respectively. Indeed, if the spectra of the precursor samples are compared with those of the samples heated at 700~ in air, a notable decrease in these two peaks are observed. The spectral decomposition of both the precursor and heated sample could allow one to compute the Si/A1 ratio and the amount of SiOM defect groups. Work is in progress to quantify the 29Si-NMR spectra. The 27Al-NMR spectra show the presence of tetrahedral A1 in structure. The thermal treatment in air at 700~ decomposes some of the tetrahedral AI and an extra-framework octahedral A1 appears in the spectra. The size and shape of the levyne crystallites of as made samples are illustrated in Figure 5 and 6. It can be seen that the size of the crystal increases with increasing A1 content in the gel. As the nucleation and the crystallization rates are decreasing with increasing A1 concentration, less nuclei are formed in the beginning of the reaction with high A1 contents, leading to the formation of larger crystals. Methylquinuclidinium ions (MQ +) are incorporated intact in the zeolite channels. The NMR lines at 58.6 and 24.9 ppm stem from CH2 groups at position 2 and 3, respectively, the 54.6 ppm line is assigned to the methyl group and the 18.8 ppm line to carbon 4 (CH group). If the spectra are taken in quantitative conditions, the relative intensities confirm these contributions. The chemical shifts of the occluded MeQ + ions are slightly influenced with respect to the solid state MeQI spectra. Indeed the chemical shifts in the latter case are
218 Table 2. 29Si-NMR results of crystalline precursor levyne samples syntesized at 150~ from gels 4.5Na20-6MeQI-xA1203-30SiO2-500H20. x
d(ppm)
Io(%)
d(ppm)
Io(%)
d(ppm)
Io(%)
d(ppm)
Io(%)
3.0 2.0 1.5 1.2 1.0 0.86
-96.7 -98.5 -98.7 -98.7 -98.7 -98.2
11.3 10.2 16.6 13.1 19.8 18.9
-103.0 -103.2 -103.3 -103.6 -103.7 -103.6
42.0 31.7 27.8 30.7 24.5 26.6
-108.8 -108.7 -108.6 -108.6 -108.6 -108.5
34.1 41.1 41.1 38.9 37.5 37.6
-115.3 -115.3 -115.3 -115.3 -115.3 -115.2
12.6 17.0 14.5 17.3 18.2 16.6
/
-90
-100
-110
-120
ppm Figure 4. MAS 29Si-NMR spectra of precursor levyne (a) and of calcined (b) sample up to 700~ in air (x=10). C2:56.7 ppm; C3:25.9 ppm; C1:19.9 ppm and CH3:54.7 ppm. The chemical shift of the methyl group ofMeQ + ions remains constant (54.4 ppm); a low field shift is observed for C-2 carbon (58.6 ppm) and a high field shift is observed for both C-3 and C-4 carbons (24.9 and 18.8 ppm, respectively). In order to identify the nature of both the low and high temperature peaks in DSC curves both 13C-NMR and mass spectrometry measurement were carried out on samples partially calcined up to 550~ It is shown unambiguously, that after the partial calcination in N2, part of the MeQ + ions is still intact in the
219
structure and the chemical shifts did not change. The spectra also show the presence.of aromatic compounds, stemming from the decomposition of the MeQ + ions characterized by the first DSC peak. Some pyridine could also be formed and a large amount of benzene can be present among the aromatic products. As a conclusion, one can say that the high temperature DSC peak contain both the MeQ + ions linked to the presence of framework negative charge, i.e. (SiOA1)-, and the decomposition products stemming from the MeQ + ions counterion to SiO" defects groups.
:.
.,,
L Figure 5 SEM micrographs oflevyne crystals obtained with SiO2/Al203 ratio 25. ..
.
,.
9
,
7,
b Figure 6 SEM micrographs oflevyne crystals obtained with SIO2/A1203 ratio 10.
220 4. C O N C L U S I O N S Highly crystalline levyne type zeolite samples are obtained from aluminosilicate gels at 150~176 in presence ofmethylquinuclidinium iodide (MeQI). The MeQ + ions are incorporated intact in the zeolitic channels and neutralize either the (SiOA1)- framework negative charges and/or the SiO" defect groups. The presence of two crystallographically different sites is confirmed by the 29Si-NMR spectra. REFERENCES
1. G. Gottardi, E. Galli, Natural Zeolites, (eds) Springler-Verlag, Berlin 1985 192. 2. W. M. Meier, D. H. Olson, Atlas of Zeolites Structure Types, ButterworthHeinemann (1992) 114. 3. Z. Tvaruzkova, M. Tupa', P. Jiru', A. Nastro, G. Giordano, F. Trifiro', Catalysis Letters, 2 (1989) 369. 4. G. T. Kerr, US Patent No 3 459 676 (1969). 5. G. D. Shorte, T.V. Wittham, Eur. Patent No 0 040 016 (1981). 6. T. R. Cannan, M. T. Brent, E. M. Flanigen, Eur. Patent Appl. No 0 091 048 A1 (1983). 7. M. T. Brent, M. T. Lok, T. R. Cannan, E. M. Flanigen, Eur. Patent Appl. No 0 091 049 A1 (1983). 8. E. J. Rosinski, M. K. Rubin, Eur. Patent Appl. No 0 107 370 (1983). 9. G. Bellussi, A. Carati, M. Millini, Ital. Patent Appl. 2 289 9A (1988). 10. A. Grunewald-Luke, H. Gies, Microporous Materials 3 (1994) 159. 11. P. Caullet, J. Patarin, A. C. Faust, in Proc. III Convegno Nazionale Scienza e Tecnologia delle Zeoliti, R. Aiello (ed), Cetraro, Italy 28-29 Sett. 1995. p.55, and P. Caullet,J. L. Guth, A. C. Faust, J. L. Loly, F. Raatz, FR. Patent Appl. N~ 9 17 163 (1989). 12. C.V. Tuoto, F. Testa, A. Nastro, Materials Engineering, 5 (1994) 175. 13. C. V. Tuoto, F. Testa, R. Aiello, A. Nastro, Atti 2 ~ Convegno Nazionale sui Materiali per Ingegneria, P. G. Orsini (ed), Trento, Italy 19-21 Sett. 2 p 173. 14. C. V. Tuoto, A. Regina, J. B.Nagy, A. Nastro, in Proc. III Convegno Nazionale Scienza e Tecnologia delle Zeoliti, R. Aiello (ed), Cetraro, Italy 28-29 Sett. 1995. p113. 15. J. Hage A1 Asswad, N. Dewaele, J. B.Nagy, R. A. Hubert, Z. Gabelica, E. G. Derouane, F. Crea, R. Aiello, A. Nastro, Zeolites, 8 (1988), 221. 16. Y. L. Casci, T. V. Whittam, Stud. Surf. Scie. Catal., 24 (1985) 39.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved. _
_
_
221
Synthesis of ETS-10 molecular sieve from systems containing TAABr salts P. De Luca and A. Nastro D e p a r t m e n t of Chemical Engineering and Materials, University of Calabria, Arcavacata di Rende, 87030 Rende (CS), Italy The synthesis conditions of the ETS-10 molecular sieve from the system a N a 2 0 - b K F - c T i O 2 - d T A A B r - l . 2 8 a H C l - l . 4 9 S i O 2 - 3 9 . 5 H 2 0 where TAABr corresponds to TMABr, TEABr, TPABr and TBABr and.0.9
222 TAABr contents and of SiO2/TiO2 ratio in the reaction mixtures. Moreover the results of thermal analysis on purified ETS-10 are reported. 2. EXPERIMENTAL The system studied was: aNa20-bKF-cTiO2-dTAABr-1.28aHCl-1.49SiO239.5H20 where TAABr corresponds to TMABr, TEABr, TPABr and TBABr and.0.9
223
'''
'I
"
'
I.
'
I
'
I
:
I
I
1.0 C~
'
I
'
1.0
o
"
#.
r~
o.4
0.4
. r"' i
ETS-4
~.~
r
0.2
0.2 I,
I
1.0
I
1
9
t
,
l
1.5 2.0 2.5 N a 2 0 , Moles
v P~''~
t
i
1.0
3.0
Figure 1. Crystallization field of the crystalline phases obtained from the system aNa20-0.6t~-cTiO2-1.28aHC]1.49SIO2-39.5H20, 0.9
9
+
0.6-
0.6
I
U'9
o
o.s
Ti407
0.8
I
oi
t
f
I
1.5, .2.0 2.5 Na20, Moles
:
!
3.0
Figure 2. Crystallization field of the crystalline phases obtained from the system aNa20-bKF,0.25TiO2-1.28aHCl1.49Si02-39.5H20, 0.9
ETS-10 is obtained in a ve~- small area, because the synthesis conditions are highly influenced by Ti02 content in the reaction batch (Figure 1). The variation of KF content in the reaction batch does not modify the area of exSstence of ETS-10 (Figure 2), and it does not produce a variation of the kinetic parameters, of the }deld of the batch and of the crystal size and morpholo~, (cubes of about 1.5 microns). The addition of any TAABr (0.2 moles) to the system aNa20-0.6KF-cTiO21 . 2 8 a H C l - l . 4 9 S i O 2 - 3 9 . 5 H 2 0 where 1.0
T,&A moles nucleation time, hours rate, %/h m~ximum yield, %
0.2 14 5.28 95
0.4 6
0.2 9
5.27 4.17 95 ~
0.4 6
0.2 6
3.46 5.22 92 94
0.4 6
0.2 9
0.4 14
2.81 93
4 . i 9 1.35 ~ 65
..... 24 1.85 89
224
.....
1.0 IID
9
0.2TMABr I
I
'
I
"
I
9
Ti407
0.8
0.8 o
0.6 ~9 0.4 0.2
"
/
i
"
li
"
i
I
.
I
.
I
"
"
Ti407 /
0.6
0.2 i
.
I
,
1.5
I
,
2.0
I
~
2.5
I
.
r "
9
I
,
1.0
3.0
I
9
1.5 2.0
2.5 3.0
Na20, Moles
Na20, Moles
0.8
|!
0.4
1.0
Q)
"
ETS-10 9
1.0
!
1.0 "0"2TEABrI
"
1.0
Ti407 / s
Ti407
0.8 o
O
N o.6
~ o.6 9 N o.4
~ 0.2
u iETS_ O \ 9
I
1.0
9
I
.
.
--'----
U
0.2 I
.
|
1.5 2.0 2.5 Na20, Moles
i
I
3.0
1.0
1.5 2.0 2.5 Na20, Moles
3.0
Figure 3. Crystallization fields of the crystalline phases obtained from the system aNa20-0.6KF-cTiO2-0.2TAABr-l.28aHCl-l.49SiO2-39.5H20, 1.0
225
1.0
1.0
0.8
0.8 ETS-10
ETS-10 0.6
0.6
0.4
~" 0.4
0.2
DTS+ETS-10 |
ETS-10+DTS DTS
DTS a
0.2
I
9
.
I
9
0.6
0.2
I
0.2
1.0
i
I"
1.0 _TPABr I
'
"
'
"
'
"
'
~
ETS-10
I i'
I
"
l
"
I
,zTs-, o.+DTs. 0.6
TAABr, Moles
"
I
ETS-10
0.6
U
0.2
I
TBABr
0.8
0.4 0.2 U
9
1.0
0.8 0.6
1.0
TAABr, Moles
TAABr, Moles 9
0.6
U
~0.4
TS-10+DTS
0.2 , I
1.0
~
0.2
I
9
I
0.6
9
I
1.0
TAABr, Moles
Figure 4. Crystallization fields of the crystalline phases obtained from the system 1.26Na20-bKF-dTAABr-0.25TiO2-1.63HCl-l.49SiO2-39.5H20, 0
226 Table 2. Chemical analysis of purified crystals of ETS-10. Water and TAA content, detected by thermal analysis, Na, K, Si and Ti per unit cell detected by EDAX. The samples are identified by the KF and the TAABr content in the reaction batch. H20/u.c. 1" 2**
SAMPLE 0.6KF
H20 %wt
TAA %wt
O.OTAABr O.2TMABr O.2TEABr 0.2TPABr O.2TBABr O.4TMABr O.4TEABr O.4TPABr O.4TBABr
14.50 10,31 6,07 5,67 4,82 8,71 4,98 3,80 6,05
.... 4.32 7.71 6.51 4.88 5.25 8.48 6.61 4.07
27,46 21,30 12,40 11,35 9,38 17,86 9,91 7,70 11,87
99,59 6,85 6,78 6,19
4.24 7.57 6.57 4,07
19,57 14,10 13,77 12,12
TAA/u.c. 1" 2**
Si/Ti Na/u.c. K/u.c.
3,43 2,66 1,54 1,40 1,17 2,23 1,29 0,94 1,48
...... 2,16 0,27 2,17 0 , 3 9 1,29 0,15 0,75 0,08 2,61 0 , 3 2 2,33 0,30 1,25 0,15 0,59 0,07
5.05 5.11 5.15 4.99 4.55 5.30 5.04 4.98 4.73
1.22 1.25 1.31 1.28 1.38 1.12 1.31 1.24 1.14
0.80 0.91 0.76 0.71 0.80 0.93 0.81 0.81 0.89
2,44 1,76 1,72 1,50
2,10 2,15 1,28 0,59
5.31 4.91 5.03 4.94
1.32 1.12 1.37 1.42
0.73 0.65 0.85 0.55
***
***
***
0.4KF O.2TMABr O.2TEABr O.2TPABr O.2TBABr
0,26 0,26 0,16 0,07
*) Results calculated on the basis of the formula Si4oTi8Olo416- (basic building block for the disordered structure) (6). **) Results calculated on the basis of the formula Si5TiO132- (stechiometry of the framework) (6). ***) Results Mean of 10 experiments on the basis of the formula Si5TiO132(stechiometry of the framework) (6). reaction gel in agreement with result of Figure 4. The results are reported in Table 1. The templating action of the tetralkylammonium salts is also confirmed by the chemical analysis data of purified ETS-10 crystals, reported in Table 2. In particular the TG data show that the water adsorbed into the pore of ETS-10 precursors, synthesized from a system without organic salt, is partially substituted by the TAA added. The TA~u.c. and the H20/u.c. detected are not constant, their amounts are a function of the molecular weight and that of the molecular size of the organic cation. The presence of TAABr in the batch composition does not substantially modify the Ti content in the crystals of ETS-10. Only higher values of Si/~ ratio are observed in the crystals obtained from systems containing TMABr. This anomalous Si/Ti ratio in the ETS-10 structure, probably, derives from the
227 combined effect of the presence of some crystalline defects, of the ability of TMA+ to produce open structures and of its hydrated size similar to hydrated Na +. More investigations are in progress to clarify this problem. The cations content per unit cell is in good agreement with the negative charges of the structure. Any inorganic anion is detected by EDAX therefore the positive charge of TAA+ cation, probably, is balanced by OH'. The amounts of Na + and K + detected are enough to balance the negative charges of the framewok. This behaviour suggests that the TAA+ cations do not replace the inorganic cations in the ETS-10 structure. These results confirm that in general the organic ions play a predominant role of pore filling. The course of DTA patterns of the different TAAETS-10 suggest the presence of one type of organic cation incorporated inside the ETS-10 channels
E X 0
-10
l
-10
AT
S-IO E N D 0
10
0
1 1 O0
! 200
1 300
1 400
! 500
! 600
700
TEMPERATURE, ~ Figure 5. DTA thermograms of the different TAAETS-10 obtained from the system:l.25Na20-0.6KF-0.4TAABr-0.25Ti02-1.6HCl-l.49Si02.39.5H20.
228 (Figure 5). In fact the thermal decomposition of TAA is connected with the single endothermal effect, its temperature is different for any type of organics. The molecular weight of TAA incorporated in ETS-10 channels plays a role on the desorbtion kinetic, in fact the resolution of the endothermic effect is more evident when the molecular weight of the TAA increases. Variation of the KF content does modify the interaction between the organic cation and the framework of ETS-10. The thermograms obtained from TAAETS-10 containing less t h a n 0.4 moles show a not well-defined effect. In agreement with the results of Table 2, the temperature of water desorption is observed at different temperatures as a function of the type of TAA incorporated inside the ETS-10 channels. More investigations are in progress to define the mechanism of ETS-10 activation. 4. CONCLUSIONS The results above reported show that the addition of a TAA+ cation to the batch composition modifies the area of existence of ETS-10 molecular sieve, and extend the range of pH where ETS-10 exists (10.0<_pH_
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
229
Synthetic clinoptilolite and distribution of aluminum atoms in the framework of l I E U type zeolites M.Kato, ~ S. Satokawa, b'~ and K. Itabashi b "Research Center for Chemometrics, Toyohashi University of Technology, Toyohashi 441, JAPAN bNanyo Research Laboratory, Tosoh Corporation, Shinnanyo 746, JAPAN
Pure (K,Na)-clinoptilolite was crystallized in good reproducibility without seed crystals. Ordered A1 distributions in frameworks of synthehized and natural clinoptilolite and natural heulandite, which are isostructural framework, were also analyzed. It was found that A1 atoms in clinoptilolite were condensed in T1 and T2 sites with space group P2/c. On the other hand, A1 atoms in heulandite were distributed in T1, T2, T3, and "I'4 sites with space group P2~, which violates against the 2 A1/5 ring avoidance rule. 1.
INTRODUCTION
There has been long discussion on the distinction between clinoptilolite and heulandite because of the difficulty of synthesis of these pure zeolite crystals in laboratory [1]. In this work, we attempted to synthesize pure (K,Na)-clinoptilolite without seed crystals. It is well known that distribution of A1 atoms in a zeolitic framework takes an important role in a catalytic activity. However, A1 distribution has been ambiguous because the atomic scattering factor of A1 atoms in XRD measurement is nearly equal to that of Si atoms. Therefore, in this work, we examined the ordered distribution of A1 atoms in natural and synthetic clinoptilolite, and natural heulandite on the basis of analysis of 298i MAS NMR spectra and their framework structures with the aid of Loewenstein's rule [2] and 2Al/5-ring avoidance rule [3], and attempted to clarify the difference between clinoptilolite and heulandite. 2. EXPERIMENTAL Materials (K,Na)-clinoptilolite was hydrothermaUy synthesized without seed crystals by homogeneous mixing of reactant mixture of (K,Na)-aluminosilicate gel during heating at 150~ for six days. Natural clinoptilolite(Na3.nKz.4Cao.7A16.6Si29.407z: Arizona, USA) and heulandite (Nal.sK0.1Ca2.9A18.6Si27.4072: Maharashtra, India) were used. Apparatus 29Si MAS NMR spectra were measured at 79.4586MHz and spinning frequency of 6 kHz with Varian Unity-400 plus spectrometer. Thermal stability was measured by TG/DTA with Rigaku Thermoflex 8100. Chemical composition of samples was determined by ICP and EDX elemental analysis. c Present address : Fundamental Technology Research Laboratory, Tokyo Gas Co. Ltd.,
Minato-ku, Tokyo 105, Japan
230 3. RESULTS AND DISCUSSIONS
3.1 Synthetic clinoptilolite Pure (K,Na)-clinoptilolite with composition of Na2.1K4.sA16.9Si29.1072 nn20 was crystallized from the reactant mixture of Si/Al=5.5, (K+Na)/Si=0.3 and K/(K+Na)--0.5. All of the diffraction peaks of the products could be assigned to those of HEU structure [4]. Pure clinoptilolite was produced within very restricted reactant composition with good reproducibility [5], and phillipsite, mordenite, or ferrierite was crystallized with clinoptilolite around the composition. The crystals of synthesized clinoptilolite have morphology like thin plate as shown by SEM photograph in Figure 1. DTA curve of natural heulandite showed two endothermic peaks at about 160~ and 300~ corresponding to dehydration [5]. In the case of synthetic and natural clinoptilolite, continuous dehydration curves in TG/DTA up to 600~ were obtained, and there was no structural change in XRD patterns after heat treatment at 600~ This phenomena agree with Figure 1. Scanning electron micrograph of synthesized the discussion of Mumpton clinoptilolite crystal. [6] that clinoptilolite structure is maintained after heating overnight at 450~ but that heulandite is decomposed in the same treatment. 3.2 NMR spectra The 29Si NMR spectrum of synthetic clinoptilolite was illustrated in Figure 2. By a peak deconvolution, four peaks(1 to 4) were obtained as shown in the figure, and the populations of Si(OA1)n(OSi)4_, (abbreviated as Si(nA1) hereafter) in the four peaks are calculated. The difference of the chemical shifts of these peaks were about 5 ppm from each other, which is almost equal to that observed in the difference of A1 number n in Si(nA1) [7]. However, if they are assigned to Si(3A1), Si(2A1), Si(1A1), and Si(0A1) from low magnetic field, the A1 content of the framework is much greater than the observed values by chemical -90 -100 -110 -120 -130 analysis. ~/ppm The chemical shift of Si atoms in the framework were reassigned on the basis of Figure 2. 29SiMAS NMR spectrum of empirical equation derived by Engelhardt synthetic clinoptilolite. [7] using the atomic coordinates of
231 tetrahedron sites (abbreviated T sites hereafter) and oxygen atoms [8]. The calculated chemical shifts were widely spread from -95 ppm to -113 ppm as illustrated in Figure 3. The chemical shift of tetrahedron sites, TI(nA1), T3((n+I)A1), and T4((n+I)A1), were almost equal value, and , , 'r:zo^l) 1 those of Tz((n+l)A1) and f rs(,^,) v,(o.,,) T4(IAI) ~ 3 _ / T4(2AI) Ts(nA1) sites were located in 2 I"~ 'r1(l^l) I a':3(2^t) both sides of them. When ~ . 'r2(2,u) } they can be divided into four 1 Ts(~^,) . . . . r~(o.,,) 4 TI(2AI)~ r - T4(0AI) groups as shown in Figure 3 which were labeled as peaks 1 to 4 from low magnetic field, it is found that the calculated chemical shifts -95 -100 -105 -UO -115 8/pi,,,, are in good agreement with the values of the observed peaks shown in Figure 2. Figure 3. Calculated chemical shifts for clinoptilolite, HEU. TS(0AI)
T2(0AI )
9
l
,
i
3.3 Ordered distribution of A! atoms in HEU type framework 3.3.1 Candidates of ordered distribution of A! atoms The framework of clinoptilolite, HEU, which was assigned to space group C2/m by Alberti [8]. However the difference between A1 and S i atoms was ignored in his assignment. So it is predicted that the assigned symmetry is higher than that of the real one. In order to distinguish A1 and Si atoms, the discussion was started from the most primitive P1 symmetry in Table 1 Configurations of eight A1 atoms in the HEU type framework, and the p 9pulation of Si(nA1). Expected intensity of peaks in Fig. 2 [Si(nA1)] Space group No. n=3 2 1 0 1 2 3 4 Configuration of A1 atoms I
TI,I* T1,2 T1,3 T1,4 T1,5 T1,6 T1,7 T],s
C2/m
0
12
8
8
4
8
8
8
II
T1,1 TI,z T1,7 Tl,s T2,3 "1"2,4Tz,5 Tz,6
P2/c
0
10 12
6
2
12
10
4
III
P2/c
0
10 12
6
6
4
14
4
P21
0
10
12
6
2
14
6
6
P21/m
0
8
16
4
4
12
8
4
VI
TI,1 T1,2 T1,7 TI,s T3,3 T3,4 T3,5 T3,6 TI,1 T1,4 T1,6 T1,7 T2,2 T2,5 T3,2 T3,5 TI,1 T1,4 Tl,6 T1,7 T3,2 T3,3 T3,5 T3,8 TI,1 T1,6 "1"2,2T2,5 T3,2 T3,5 %,4 T4,7
P21
0
10 12
6
2
14
8
4
VII
T2,1 T2,2 T2,5 T2,6 T3,1 T3,2 T3,5 T3,6
C2
0
12
8
8
4
12
8
4
VIII T2,1T2,2 T2,7 T2,s "1"3,3T3,4 T3,5 T3,6
P2/c
0
8
16
4
4
8
16
0
T2,1T2,3 .T2,6 Tz,s T3,1 T3,3 T3,6 T3,8
P2a/C
0
12
8
8
4
12
8
4
T2,1 "1"2,6%,1 T3,2 T3,3 T3,s T3,6 T3,s
P21
0
10
12
6
6
6
14
2
IV V
IX X XI
T3,1 T3,2 T3,3T3,4 T3,5 T3,6 T3,7 T3,s C2/m 0 8 16 4 8 0 20 0 *In Ti,/, i corresponds to the site in Ref.[8] andj the number of the equivalent position of Ref. [10].
232 of atomic coordinates by the same manner described in previous papers [3,9]. Using the connectivity table, candidates of ordered distribution of A1 atoms in the HEU type framework were searched under the restriction of Loewenstein's rule and 2A1/5-ring avoidance rule proposed in the previous paper [3]. Some of the candidates with high symmetry were listed in Table 1 out of hundreds of them, along with the calculated population of Si(nA1) and the expected intensity of the peaks 1 to 4 in the 29Si MAS NMR spectra. It is found from the table that the maximum Figure 4. Projection to bc-plane of ordered number of A1 atoms in the framework is eight per unit cell. The A1 content per unit distribution of A1 atoms in clinoptilolite with cell observed in most of natural space group P2/c. @ 9A1. clinoptilolite is in good agreement with this value. In order to contain more than eight A1 atoms per unit cell in the framework, the A1 distribution must violate against the 2 Al/5-ring avoidance rule. Also, it is shown that Si(3A1) cannot exist in the framework except for only one configuration with space group P1. 3.3.2
Clinoptilolite
The ordered distribution of A1 atoms in the framework must satisfy the observed 298i MAS NMR spectra and A1 atoms should be condensed in "I'2 site [8,10]. In the candidates listed in Table 1, the configuration with P2/c (P12/al in non-standard form) symmetry (No. II) was selected. In the ordered distribution, A1 atoms are located in TI.~ T1,2 TI,7 Tl,s T2.3 T2.4 T2.5 and T2.6sites shown in Figure 4. Real crystals of clinoptilolite contain less A1 atoms than eight for the ideal distribution. Therefore, substitutions of A1 atoms by Si atoms in the framework must be considered. The substitutions are summarized in Table 2 along with the population change of [Si(nA1)] in five To sites and A1 content. The peak intensities were calculated from the ideal populations and their changes by these substitutions. The results were listed in Table 3. It is found that the calculated intensities agree well with the observed intensities. This means that a misplacement of A1 atoms in the framework is almost negligible, because only the substitutions of A1 atoms by Si atoms were considered in this calculation. A1 atoms are ideally located in T1 and "I'2sites. In these sites, A1 atoms in T1 sites are easily substituted by S i atoms in real crystals, and occupation of A1 atoms in the site decreases from 50 % to 37%. On the other hand, A1 atoms in "I'2sites are hardly substituted, and the occupation is ca 45%. The value of occupation in T2 site is in good agreement with the value estimated from XRD data by Alberti [8]. It is reported that cations in clinoptilolite are located near T2 site [8,10], Which also agree with the model of ordered distribution of A1 atoms of this work In XRD measurements, space group C2/m [8,10] has been assigned to the framework of clinoptilolite. The space groups P2/c proposed in this study have lower symmetry than C2/m,
233 Table 2 of NMR spectrum by substitution of A1 atom Si in clinoptilolite. Peak no. 1 2 3 n in Si(nA1) 2 2 2 2 1 2 1 mill 0 l ! l l l ~ Site T1 Ts T2 T3 T1 T4 Ts Ideal population of [Si(nA1)]/u.c. 0 2 4 4 4 0 0 Population changes by -1 substitution in T2 site(Si) -1 +1-1 +1-1 -1 -2 -4 substitution in T1,7 and Tl,s sites(Sa) +2 +4 +2 +1 +2 +2 +2 -2 -2 -2 substitution in T1,1 and T1,7 sites(Sin) +, - 9indicate the population changes relative to the ideal
4 [AI] 0 0 /u.c. T 2 T 3 T4 004 8 0
+1 +1 +1 -1 -2
,.
+2
-2
Table 3 Observed and calculated NMR spectra of clinoptilolite. peak No. Synthesized clinoptilolite 0.49x Sn+ 0.11 x SI observed Acalc-obs Natural clinoptilolite 0.26 x SI + 0.53 x Sn+0.05 x Sm observed Aca|c-obs
1
[Si(nA1)]/u.c. 2 3
4
[A1] /u.c.
1.5
8.8
14.4
4.3
6.9
1.6 -0.1
8.8 _+0.0
14.2 +0.2
4.5 -0.2
6.91 -0.01
1.4 1.2 +0.2
8.2 8.0 +0.2
15.0 15.2 -0.2
4.9 5.1 -0.2
6.5s 6.58 :tO
but one of the subgroups of C2/m. The configuration of A1 atoms presented here has always the topologically same structure, e.g., the configuration of (T1,3, T1,4, T1,5, T1,6, T2,1, T2,2, T2,6 and T2,8 ) is topologically the same as the configuration of (TI,1, T1,2, T1,7, T1,8, T2,3, T2,4, T2,5 and T2,6). In real crystal, both of these configurations should be realized with equivalent probability. Therefore the space group determined by XRD can be higher than the space group assigned by the consideration of the ordered distribution of A1 atoms. In this case, eight sites of T1 and T2 which are divided into two groups in space group P2/c become equivalent, and apparent space group in XRD measurement becomes C2/m. 3.3.3 Heulandite In the above configuration for clinoptilolite, there are two sites which can be occupied by additional A1 atoms. However the calculated intensities of the peaks of NMR spectrum for heulandite did not agree with the observed one, where chemical shifts calculated using the atomic coordinates reported by Alberti [11] were almost equal to those of clinoptilolite. So another configuration for heulandite must be selected from the candidates listed in Table 1, since typical A1 content per unit cell of heulandite in natural samples [ 1] is reported as nine and has not exceeded ten, which is very close to the value of clinoptilolite. If the Loewenstein's rule is only one restriction of distribution of A1 atoms, more A1 atoms should be contained in the framework. The candidate of ordered distribution of A1 atoms should satisfy that expected intensity of peak 1 should be less than four because the observed population was 3.6 and it should
234 increase when A1 atoms inserted. Consequently the ordered configuration illustrated in Figure 5 was selected as a candidate, whose symmetry is P21. The configuration was derived from configuration VI in Table 1 which is inserted two Al atoms into T2,~ and "1"2,6sites. Ten A1 atoms are contained in the ideal distribution, and they are located at T~,~, T1.6, T2,1, "1"2,2,"1"2,5, "I'2,6, T3,2, T3,5, "1"4,4,and T4,7 sites. In the configuration, no more Al atoms can be inserted by the restriction of Loewenstein's rule, that is, the number of Al atoms is limited to 10 per unit cell in heulandite [ 1]. In order to compare with a real crystal, the substitutions of A1 atoms by Si atoms were considered as clinoptilolite. The population changes of Si(nA!)s are T: summarized in Table 4. The calculated peak intensities were in good agreement with .2 the observed values as listed in Table 5. T ~,7 Although extra A1 atoms were added to T2 L sites, the substitution is occurred at T1 and . T3 sites. Consequently, in heulandite, A1 atoms are condensed in "/'2 sites ! (occupation is 50%), and small amount of A1 atoms distributed in T1 (16%), T3(16%), and "1"4(25%) site. Alberti [ 11] concluded from the bond distances between T site and oxygen site that occupancy of A1 atoms in "I"2 Figure 5. Projection to be-plane of site atoms was about 40%, and 25% in T1, "1"3 and T5 sites. On the other hand, configuration of Alatomsinheulandite. Markle and Slaughter [12] concluded that A1 @ 9Al atoms. atoms were mainly co_ndensed in T2 (50%) and "1"4sites (50%), and small amount of Al atoms is in T1 site (13%) in notation of space group C2/m ( they refined the structure in space group Cm). Their conclusions agree .....with the present results from the view point of the condensation of A1 atoms in T2 site. It is reported that cations in heulandite are located near T2 site [11], which also agree with this work. The A1 content of heulandite is greater than eight per unit cell predicted from the 2 A1/5ring avoidance rule. It means that heulandite violates against the rule. Moreover, the Table 4 Chan of NMR s~ substitution of A1 atom b, Si in heulandite. Peakno. 1 2 3 4 [A1] n in Si(nA1) 3 3 2 3 2 2 2 1 2 1 1 1 0 1 0 0 0 0/u.c. Site T2 T3 T1 T4 T5 'I'2 T3 T1 '1"4 T5 T~ T2 T3 T1 "I'4 T5 T2 T3 "I'4 Ideal population of [Si(nAl)]/u.c. 2 2 2 0 0 2 0 4 2 4 ~DmHwmmm~ Population changes by substitution inT1 site(Sin) -1 -1 +1 +1 -1 ma,mmmmmmm substitution in T3 site(S~) 0 -1 -1 -1 mmmmmmmmmlm +, - 9indicate the population changes relative to the ideal
235 ordered configuration of A1 atoms differs Table 5 from that of clinoptilolite. These Observed and calculated NMR spectra of natural difference seems to be the reason that heulandite thermal stability of heulandite is lower than [Si(nAl)]/u.c. [AI] that of clinoptilolite. Peak No. 1 2 3 4 /u.c. The occurrence of heulandite shows 3.9 11.3 10.8 1.4 8.6 0.7 x (Sin + San) that 2 Al/5-ring avoidance rule may be observed 3.6 11.8 11.1 1.0 8.6 weaker restriction of A1 distribution than +0.3 -0.5 -0.3 +0.4 __+0.0 Aeale-obs the Loewenstein's rule. In the case of heulandite, driving force of the violence against the rule seems to be a charge compensation of Ca cation by A1 atoms in the framework.. 4. CONCLUSIONS Clinoptilolite can be synthesized from very narrow region of reactant mixture with good reproducibility without seed crystals. In the framework of clinoptilolite, eight A1 atoms are theoretically ordered in T1 and I'2 sites with space group P2/c. Heulandite has the same framework as clinoptilolite, and 10 A1 atoms are located in T~, T2, T3, and '1"4sites. In both zeolites, A1 atoms mainly occupy "I"2site. It is considered that the thermal instability of heulandite against clinoptilolite is attributed to the violation against 2 A1/5-ring avoidance rule. Acknowledgment
The authors thank Prof. T. Takaishi for his helpful suggestions. References
1. G. Gottardi and E. Galli, Natural Zeolites, Springer-Verlag, Berlin 1985. 2. W. Loewenstein, Am. Mineral., 39 (1954) 92. 3. T. Takaishi, M. Kato and K. Itabashi, Zeolites, 15 (1995) 21. 4. W.M.Meier and D.H.Olson, Atlas of Zeolite Structure Type, Butterworth-Heinemann, Stoneham, 1992. 5. S. Satokawa and K. Itabashi, to be submitted. 6. F.A.Mumpton, Am. Mineral., 57 (1972) 1463. 7. G. Engelhardt, Proceedings of 1989 Meeting of British Zeolite Assoc., (1989) 151. 8. A. Alberti, Tschrmaks Min. Petr. Mitt., 22 (1975) 25. 9. T. Takaishi and M. Kato, Zeolites, 15 (1995) 689. 10. K. Koyama and Y. Takeuchi, Z. Kristallogr., 145 (1977) 216. 11. A. Alberti, Tschrmaks Min. Petr. Mitt., 18 (1972) 129. 12. A.B.Markle and M. Slaughter, Amer. Mineral., 53 (1968) 1120.
This Page Intentionally Left Blank
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 1997 Elsevier Science B.V.
237
Preparation of ultramarine analogs from zeolites S. Kowalak, M. Str6~,yk, M. Pawtowska, M. Milu~ka and J. Kania Adam Mickiewicz University, Faculty of Chemistry, ul. Grunwaldzka 6, 60-780 Poznafi, Poland
Novel methods for ultramarine analogs preparation involving generation of sulfur radicals inside the synthetic zeolites are presented. Sulfur compounds were introduced into the zeolites porous structures either by impregnation or hydrothermal treatment or even during crystallization of zeolites in their presence. The samples were then calcined for short time in order to generate the radicals. Oppositely to conventional syntheses of ultramarine the emission of SO2 was found negligible. INTRODUCTION The technology of the artificial ultramarine production has been developed as early as in 1820's independently by J.B. Guimet in France and C. G. Gmelin in Germany [ 1]. The largescale production started in Germany already in 1830. The technology consisted in calcination of mixtures of kaolin, sodium carbonate, elemental sulfur and reducting agents for long time (at least one week) at high temperature (800~ or higher). The inexpensive substrates and the simple technology made the resulting ultramarine a very cheap and common product. The production raised very fast and almost one hundred factories producing ultramarine were operating in Europe in the beginning of twentieth century. The technology did not change considerably until now. The main drawback of this method is the presence of large amount of sulfur dioxide in waste gases. About one half of the total sulfur in the substrate mixture is transformed into SO2 upon calcination. The contemporary regulations on environment protection can not accept the pollution resulting from this production. Neutralization of sulfur oxides is complicated and expensive. Although ultramarine is still a product of high market demand, most of the factories in Europe closed, because of the pollution problem. Both, natural (Lazurite, Lapis lazuli) and synthetic ultramarine show the structure of sodalite. The anion-radicals $3-, responsible for the intense blue color, are sitting inside the sodalite cages (6.4A in diameter) which are very suitable for their accommodation [2]. Encapsulation of sulfur radicals inside the 13-cages provides their stability and subsequently makes the ultramarine blue an extremely durable dye. The sodalite cages are part of the structure of several molecular sieves (LTA, FAU) as secondary building units. It seemed reasonable that
238 the 13-cages of most common commercial zeolites such as A, X, Y, could be also adequate to encapsulate the sulfur radicals. The first attempts to use zeolites for the preparation of ultramarine have been already reported in the beginning of the 1950's [3-5]. The conventional synthesis of ultramarine consists in a high temperature crystallization of sodalite structure with a simultaneous generation of the sulfur radicals inside its cavities. It is likely that the introduction or generation of the radicals inside the porous structure of zeolites could be carried out at much milder conditions. The gentle condition should prevent a high emission of sulfur oxides. We have undertaken several approaches to prepare ultramarine analogs from zeolites. The anion-radicals S3- identical to those found in ultramarine have been obtained by dissolving certain alkali polysulfides in electron pair donor solvents such as DMSO, DMF, NH3 [6-8 ]. We tried to introduce the radicals into zeolites from DMSO or liquid NH 3 solutions of Na2S 3. The results have not been very promising so far [9]. The blue color of impregnated zeolites vanished upon evacuation of the solvent and the ESR spectra did not indicate the presence of S3- radicals in the resulting samples. Generation of radicals in zeolites from precursors introduced into zeolites has appeared as a more suitable approach. The precursors such as sodium sulfides or polysulfides have been incorporated by impregnation of zeolites [ 10,11 ]. The samples were then calcined for several hours either at high temperatures (above 500oc) in the presence of a reducing agent (coal tar) or at a relatively low temperature (350oc) without any reducing agent. In another series of experiments the impregnation was replaced by a hydrothermal treatment of zeolites with aqueous precursor solutions in an autoclave at elevated temperatures (100 -200oc). The obtained samples usually showed a light blue color which turned deep blue after a short calcination [ 12]. Another approach comprised a crystallization of zeolites (A,X, hydroxysodalite) in the presence of sulfur compounds in order to incorporate them into the intracrystalline cavities already on nucleation of the zeolite structure. This method of encapsulation has been proved successful for various metal complex compounds [ 13]. The crystallization products were then heated to generate the sulfur radicals. The crystallization mixture was mostly obtained from sodium silicate and aluminate. In some experiments kaolin was used as starting material for crystallization [ 14]. Kaolin was also employed in other experiments similar to traditional ultramarine synthesis. The main difference was the use of sodium sulfide or polysulfide in the substrate mixture instead of elemental sulfur. The formal charge of the anion-radical S3- is -1/3. Thus, the use of negatively charged sulfur compounds should be advantageous to reach the formal charge value of-l/3 in the oxidative condition of thermal procedure. This can also prevent the total oxidation of the sulfur compounds to sulfur dioxide which always occurs in the conventional method [ 15]. Besides the experiments of commercial interest we have also studied thermochromic effects with ammonium polysulfide [ 16], the influence of cation zeolite modification on generation of sulfur radicals [ 17] and AIPO4-20 ultramarine analogs [ 18 ]. The following work summarizes some results of our previous study [9,10, 11, 14,15, 16] and presents the new data.
239 2. EXPERIMENTAL The commercial zeolites NaA, NaX, NaY supplied by SODA, Ma,twy, Poland, Na mordenites (Leuna Werke) and Na ZSM-5 ("Ultrazet" from Institute of Industrial Chemistry, Warsaw) were used as principal parent materials. We also used hydroxysodalite, AIPO4-5 [19] and AIPO4-20 [20 ] prepared in our laboratory according to published recipes. Kaolin (A1203-32,5%, SIO2-53,7% ) was supplied by Otdrzychrw mine, Poland and Na2S. 91-120 by POCH, Poland. Elemental sulfur was provided by Siarkopol, Poland. The impregnation of molecular sieves (NaA, NaX, NaY, Na-hydroxysodalite, Na-mordenite, Na-ZSM, AIPO4-5, A1PO4-20) has been carried out using an incipient wetness technique. Polysulfide Na2S 3 was mostly used in the preparations presented in this study. It has been obtained by merging Na2S with adequate amounts of elemental sulfur. The quantity of sulfur introduced as polysulfide constituted 15 wt.% of the whole composite material. The impregnated samples were dried at 100~ Then the reducing agent, coal tar, was admitted (1/5 of zeolite weight) and then they were calcined in covered ceramic crucibles at temperatures 500-850~ for two hours. The samples were heated for additional two hours in open crucible at 600~ In other experiments impregnated samples were heated without any reducing agent at 350~ for two hours. Hydrothermal treatment of zeolites was carried out in Teflon lined autoclave at temperatures ranging from 100 to 200~ for 22 hours. Zeolites were immersed in concentrated aqueous solution (-~30%) of Na2S 3. The number of sulfur (as Na2S3) was about 15 wt.% of the zeolite. The samples were then filtered, washed and dried at 100~ Finally they were calcined at 800 ~ C for 15 minutes without any reducing agent. Crystallization of zeolites (A,X, sodalite) was conducted under conventional condition [19]. The composition of the initial mixtures was however completed by various amounts ofNa2S 3 (Table 3). The initial aluminosilicate gel was formed from sodium aluminate and silicate solutions. Some preparations were conducted with kaolin and NaOH as crystallization substrates. In other experiments elemental sulfur replaced sodium polysulfide. The samples after synthesis were washed with water and dried and then calcined with a reducing agent similarly as for impregnated zeolites. The conventional thermal method of ultramarine synthesis has been modified by using sodium sulfide or polysulfide instead of elemental sulfur. The substrates were ground together with coal tar and calcined in covered crucibles at 850~ for 3 hours and then additionally heated in full contact of air at 600~ The color of the samples under study was estimated visually. The electronic spectra were recorded on Shimadzu UV-160 spectrometer, using glycerine suspension and they were compared to those of commercial ultramarine (produced by Reckitt's Colours or Polifarb). Crystallinity was measured by XRD (TUR M-62). ESR spectra have been recorded at room temperature (Radiopan EPR Spectrometer, 9.4 GHz, magnetic modulation 100 KHz), the g value was estimated by calibration of magnetic induction and microwave freqency. Thermogravimeric analyses were conducted in static air atmosphere (Derivatograph MOM OD- 102).
240 RESULTS AND DISCUSSION
Introduction of anion-radicals S 3- into zeolites NaA and NaX from DMSO and liquid ammonia solutions did not result in ultramarine analogs [9]. It is very likely that solvated radicals approach only the large cavities. Evacuation of the solvent causes their transformation or recombination before reaching the 13 cages. Although the ESR indicated the presence of some radical species but these were certainly not the S3" radicals. Table 1 Results of impregnation of zeolites with Na2S 3 followed by calcination at various temperature Parent zeolite Calcination Color Final structure temperature (XRD) NaA 850~ deep blue SOD 650~ blue SOD+LTA 500~ light blue LTA+SOD 350~ * blue LTA 850~ intense blue SOD NaX 650~ light blue SOD+FAU 500~ very light blue FAU+SOD 350~ * white FAU 850~ grey blue SOD NaY 650~ grey blue SOD+FAU 500~ very light blue FAU+SOD 350~ * light blue FAU 850~ dark blue SOD Hydroxysodalite 650~ blue SOD 500~ light blue SOD 350~ * light blue SOD 850~ grey almost Na-ZSM-5 amorphous 850 ~ grey amorphous Na-mordenite 850~ light blue SOD AIPO4-20 * calcined at 350 without a reducing agent Table 1 shows that most of the parent molecular sieves impregnated with sodium polysulfide (Na2S3) show a blue color similar to that of ultramarine, after short calcination. It is significant that the blue color is attained only for the molecular sieves containing sodalite cages (A, X, Y, sodalite and AIPO4-20 ). It seems the 13 cages are very important for generation and stabilization of the radicals. Although the color of modified AIPO-20 is less intense than that of zeolites it is remarkable that the same geometry of the host matrix provokes encag
241 ing the radicals, regardless their composition. Zeolites involving a channel pore system (mordenite and ZSM-5) do not turn blue upon modification. Although sodalite cages are very suitable to accommodate radicals, there are also reports [21,22] that other cavities (e.g. of zeolite P) can be filled with sulfur radicals and form ultramarine analogs. Table 1 shows that high temperature treatments of impregnated zeolites results in structural transformations. 612 g
2.0286
1
/
' 3
9 605 605 2.0292
200
600
1000 nm
Fig. 1 Electronic spectra of: 1. Ultramarine Reckitt's, 2. Zeolite 13X hydrothermally treated with Na2S 3 and calcined at 800~ 3. Zeolite 4A after the same modification, 4. Zeolite 13X after hydrothermal procedure, 5. Zeolite 4A after hydrothermal procedure, 6. Zeolite Y impregnated with Na2S 3 and calcined at 350~
320
~
330
S
340 B[mT]
Fig.2 ESR spectra of." 1.Ultramarine Reckitt' s, 2. Zeolite 4A, impregnated with Na2S 3 and calcined at 850~ 3. Zeolite 4A after hydrothermal process, 4. Zeolite 4A hydrothermally treated with NazS 3 and calcined at 800~ 5. Zeolite 4A impregnated with Na2S 3 and calcined at 350~
The sodalite structure is detected noticeable in modified zeolites A and faujasites already after calcination at 500~ The contribution of SOD structure increases with temperature and it becomes the only crystalline phase aider calcination at 850oc. Neither the ordinary calcination of the parent zeolites of these types nor those impregnated with NaOH leads their transformation into the SOD structure. It therefore seems that the sulfur compounds are
242 responsible for directing the recrystallization, which means they act as templates. They probably play similar a role in the conventional thermal crystallization of ultramarine. It is conceivable that the sodalite cages filled with sulfur derivatives do not undergo the decomposition before the recrystallization but they are rather rearranged upon calcination towards sodalite. Zeolites ZSM-5 and mordenite (that do not involve cages ) undergo an amorphization upon thermal treatment. Recrystallization of zeolites A and X in the presence of sodium polysulfides is already noticeable up on hydrothermal modification in autoclave above 180~ (Table 2). Recrystallization can result from increased sodium amount or from templating effect of sulfides. The samples treated at 195oc show a light blue color. Table 2. Properties of zeolites hydrothermally treated with Na2S3, followed by calcination at 800~ Zeolite Autoclave Structure before Color before Color a~er temperature calcination calcination calcination A 100~ LTA white white 150~ LTA light green white 195~ SOD white deep blue X 100~ FAU white white 150~ FAU white white 195~ SOD light blue deep blue Table 3. Results of zeolite crystallization in the presence of Na2S3. Zeolite Molar ratio Structure Si: AI:Na: S :H20 A, 85~ 4h 1:1:2:0:20 LTA 1:1:3.2:1.8:20 LTA+SOD 1:1:4.4:3.6:20 SOD+LTA X, 90~ 14h 1.5:1:3.5:0:145 FAU 1.5:1:4.5:1.5:145 FAU+SOD 1.5:1:6.7:4.4:145 SOD+FAU Sodalite, 95~ 25h 1.5:1:2.8:0:34 SOD 1.5:1:3.1:0.5:34 SOD 1.5:1:3.7:1.4:34 SOD Sodalite (kaolin), 1.4:1:1.9:2.8:20 CAN 195~ 23h 1.4:1:3.8:5.7:20 CAN "1.4:1:2.7:5.9:25 CAN * elemental sulfur
Color atter calcination white light blue light blue white light blue blue white lisht blue blue blue blue blue
The presence of S 3- radicals was confirmed by ESR (Fig. 2). Short (15 min.) heating leads to a very deep blue color (Fig.l). Calcination of polysulfide impregnated zeolites (A, X, Y) at
243 350oc without reducing agents results in light blue products of the retained zeolite structure. Their ESR signal anisotropy can result from the extra cage $3" radicals. Crystallization of zeolites in the presence of various amounts ofNa2S 3 followed by calcination gives rise to a blue product of relatively low color intensity (Table 3). Small amounts of polysulfide introduced do not affect the crystallization and the parent structures (LTA or FAU) are maintained, but most of sulfur compounds is washed out atter synthesis. Calcination of such samples results in colorless products. Increase in polysulfide content causes the formation of sodalite. The latter becomes the predominant structure for high they Na2S concentration. Such a direction of crystallization can result from increased Na2S 3 contents reflecting a templating effect of the polysulfide. Kaolin resulted mostly in cancrinite atter a crystallization and then turned to SOD upon calcination.
L ....
n A
I I
TG
I I
0,5%..
DTA 9
100
500
900~
100
,
,
] |
I 500
900 ~
Fig. 3 Thermogravimetric curves of conventional mixture (kaolin, S, Na2CO3),-A and zeolite 4A impregnated with NazS3.-B. Modification of the traditional ultramarine synthesis by using sodium sulfide of polysulfide results in product of similar quality as produced with elemental sulfur. Emission of SO 2, however, is several times lower. Thermogravimetric curve of zeolites impregnated with polysulfide (Fig. 3) shows that the weight loss caused by evolving SO2 is almost negligible. CONCLUSION Ultramarine analogs can be produced from zeolites under much milder conditions than those used in conventional technologies. It allows to significantly reduce the SO2 evolution. Impregnation of zeolites (particularly these involving sodalite cages in their structure) with sulfur radical precursors followed by short calcination results in products comparable to synthetic ultramarine. High temperature calcination causes transformation of zeolites A, X and .Y into sodalite. Mild calcination results in light blue products of unchanged structure. The above procedure was also successful for generation of sulfur radicals in AIPO4-20.
244 Hydrothermal treatment of zeolites A and X with Na2S in autoclave at elevated temperatures gives rise to their recrystallization to sodalite. A certain amount of radicals is generated during this procedure. Further calcination yields intense blue products. Crystallization of zeolites in the presence of polysulfides or elemental sulfur followed by further calcination results in ultramarine analogs of relatively low color intensity. The sulfur compounds affects the crystallization and facilitates the formation of sodalite or of cancrinite. Conventional synthesis of ultramarine can be modified by replacing elemental sulfur by sodium sulfide or polysulfide. This modification provides substantial reduction of SO2 emission.
Acknowledgement We acknowledge a support from the Polish Committee for Science Research (grant 7 $203 051 05). REFERENCES 1. F. Seel, Studies in Inorganic Chemistry, 5 (1994), 69. 2. G.D. Stucky, V.I. Srdanov, W.T.A. Harrison, T.E. Gier, N.L. Keder, K.L. Moran, K. Haug, and H.I. Metiu, T. Bein (eds.), ACS Symposium Series 499, (1992), 294. 3. A.E. Gessler, S. Kumins and C.A. Kumins, U.S. Patent 2535 057, (1950). 4. C.A. Kumins, U.S. Patent 2535 057, (1951). 5. C.A. Kumins and A.E. Gessler, Ind. Eng. Chem., 43,(1953),3. 6. F. Seel, G. Simon, J. Schuh, M. Wagner, B. Wolf, L. Ruppert and A.B. Wi~ckowski, Z. Anorg. Allg. Chem.., 536, (1986), 177. 7. V. Pinon, E. Levillain and J.P. Lelieur, J. Mang. Reson., 96, (1992), 31. 8. P. Dubois, J.P. Lelieur and G. Lepoutre, Inorg. Chem., 27, (1988), 73. 9. S. Kowalak, M. Pawtowska, M. Milu~ka, M. Str62yk, J. Kania, W. Przystajko, Colloids and Surfaces A,101, (1995), 179. 10. S. Kowalak, M. Milugka, A.B. Wi~ckowski and J. Goslar, Mol. Phys. Rep., 5, (1994), 223. 11. S. Kowalak, Polish Patent pending, P-302065,(1994). 12. S. Kowalak, M. Str62yk, J. Kania, to be published. 13. K.J. Balkus, S. Kowalak, U.S. Patent 5,167,942, (1992). 14. J. Kania, M. Str62yk, M. Pawtowska, S. Kowalak, in Characterization and Properties of Zeolitic Materials, M. Rozwadowski (eds), N. Copernicus Univ. Press, Torufi, (1994), 43. 15. B. Gliniany, S. Kowalak, ibid., 49. 16. S. Kowalak, M. Str62yk, J. Chem. Soc. Faraday Trans. in press. 17. S. Kowalak, M. Str62yk, M. Wr6bel, in preparation. 18. S. Kowalak, M. Pawtowska, M. Str62yk, to be published. 19. D. W. Breck, Zeolite Molecular Sieves, Wiley, New York, (1974). 20. M. Szostak, Molecular Sieves, Van Nostrand Reinhold Catalysis Series, New York (1989). 21. W.D. Galstian, A.K. Nadjarian, S.S. Karakhanian, E.B. Oganiesjan, F.S. Szakhazarian, S.A.Grigorjan, S.U.Patent 1638147 A1, (1984). 22. S. Kowalak, J. Matycha, to be published.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105. 9 1997 Elsevier Science B.V. All rights reserved.
245
E x p l o r a t i o n of n o n c o n v e n t i o n a l routes to synthesize M F I type titano- and (boro-titano)- zeolites M. Shibata*, J. G6rard and Z. Gabelica Facult6s Universitaires de Namur, I)6partement de Chimie 61, Rue de Bruxelles, B-5000 Namur, Belgium A wide series of non conventional, simple, rapid and inexpensive synthesis routes to prepare well crystallized (Ti)- and (Ti,B)-MFI zeolites from short chain alkylamine media have been explored. A new procedure involving an in situ seeding phenomenon was successfully used to considerably accelerate the crystallization. Ti is readily incorporated into the MFI framework, either alone or along with boron, as confirmed by XRD, IR, UV-vis and NMR techniques. Both ions show a homogeneous distribution throughout the zeolite crystallites grown in the presence of methylamine. B-Ti concentration gradients could appear when methylamine is admixed with fluoride ions used as co-mineralizing species. 1. I N T R O D U C T I O N MFI type titanosilicates have been shown to be excellent catalysts in various reactions involving olefin epoxidation and hydroxylation with hydrogen peroxide [1]. On the other hand, most of the known (M)-MFI zeolites (where M stands for a trivalent ion such as A13+, Ga 3+, B 3+... thus generating Br6nsted type acidic sites) are currently used in acid catalyzed reactions. It was recently anticipated [2,3] that mixed (Ti,M)-MFI materials would behave as bifunctional catalysts for both types of reactions. In that respect, the presence of milder acidic centers like the bringing hydroxyls induced by B 3+ ions within the titanosilicate framework, is expected to synergize the overall oxidation properties of such catalysts [3,4]. An efficient incorporation of Ti in the MFI framework requires quite severe preparation conditions such as, for example, the absence of any trace of alkali cations. Consequently, the various routes leading to (Ti)-MFI or (Ti,B)-MFI necessarily involve the use of elaborated and cosily reactants such as for instance various Ti-alkylates and alkali free TPAOH. The aim of this work was to explore a series of more readily accessible, less time consuming and inexpensive alternative routes, yielding both (Ti)- and (Ti,B)- MFI zeolites. The preparation procedures described here are based on the use of alkali free mineralizing agents such as methylamine. This compound was shown to efficiently mobilize through complexation a wide series of metallic ions [5]. Moreover, it does not compete with TPA for the templating role in crystallizing MFI zeolites. Finally, its basic properties represent the advantage, not only to solubilize silica, but also to use of alkali free tetrapropylammonium bromide (TPABr) instead of using the costly tetrapropylammonium hydroxide (TPAOH) [6].
* Present address: Kao Corporation, Tokyo Research Laboratories 1-3, Bunka 2-chome, Sumidaku, Tokyo 131, Japan
246 We also wanted to test a recently elaborated method that consists in adding ingredients into an already preheated gel precursor to silicalite, in which a very low amount of silicalite crystals were already generated from preliminary heating. This procedure was designated as the in situ seeding method because the silicalite crystals were shown to act as true fresh seeds dramatically accelerating the crystallization of various MFI metallosilicates [7].
2. EXPERIMENTAL 2.1 Synthesis of titanosilicates and boro-titanosilicates The short chain amine used as the mineralizing agent was methylamine (aq. 40% from Fluka). Alkali-free TPABr (Janssen Chimica) was used as a template for the MFI structure. Titanium tetrachloride (Merck) and boric acid (UCB Chemicals) were the main Ti and B reagents respectively. Although SiC14 can be advantageously co-hydrolyzed with TiC14 so as to yield homogeneous Si-Ti hydrogels [8], fumed silica (Aerosil 200 from Degussa) was preferentially used in order to accelerate the crystallization process. Some other potential complexing agents towards titanium, namely hydrogen fluoride, hydrogen chloride and oxalic acid, were optionally added to the initial gels. Two procedures for preparing the reaction gel were selected.
i) Conventional synthesis Titanium tetrachloride was carefully added to an aqueous solution of TPABr and boric acid which was cooled to 5~ beforehand. A complexing agent was optionally added to the solution. After adding SiO 2 in small portions, the resulting gelatinous suspension was admixed with methylamine. Optionally, ground silicalite crystallites were added as seeds to the reaction gel.
ii) In situ seeding synthesis Titanium-free borosilicate or silicate gel were prepared similarly to the above described method and heated at 185~ for 6h in autoclaves. The so-obtained intermediate phase (gel and about 3-5 wt. % of borosilicate or silicalite crystals generated "in situ" and considered as "seed" ) was cooled to ambient temperature and then mixed with TiCI4, prior to a second heating step. The reaction gels prepared by the both methods were heated at 185~ for several days in Teflon coated stainless steel autoclaves, in static conditions. The final solids were filtered, washed thoroughly with cold water and then dried at 100~ for 12h. More detailed synthesis conditions and some properties of the various crystalline phases are summarized in Table 1. For products still containing residual amorphous phase after heating (thus that were not 100% crystalline), the unreacted gel could be removed by achieving phase separation with the help of an ultrasonic generator (ultrasonic washing), before measuring some characteristic properties of the pure crystals, such as their composition by EDX analysis or lattice constant determination. Calcination was performed under nitrogen (heating rate: 10~ from 20 to 550~ the samples were further maintained at 550~ for 6h in flowing air prior to cooling.
2.2 Characterization All the products were checked for their nature and purity by SEM (Philips XL 20 electron microscope). Spot EDX quantitative analysis of Si and Ti on selective areas (core and edge) across individual crystallites was performed using an EDAX P.V. 9800 Phillips analyzer coupled with SEM. X-ray powder diffraction patterns were recorded on a Philips P.W. 1349 / 30 diffractometer (Cu-K0~ radiation) using a-alumina as internal standard. Crystallinities were also determined by probing the internal pore volume by n-hexane adsorption at 90~ within a
247 Stanton Redcroft ST-780 thermobalance (simultaneous TG-DTA-DTG), as described previously [9]. FT-IR spectra were obtained using a Bio-Rad FTS-60A spectrometer with KBr pellets containing 1 wt. % sample. UV-vis spectra were recorded by a Shimadzu UV-3100PC spectrometer. ~IB-MAS NMR spectra were recorded on a Bruker MSL-400 spectrometer. The detailed experimental conditions for NMR were described elsewhere [ 10]. 3. RESULTS AND DISCUSSION 3.1 Crystallization of titanosilicates While 100% crystalline silicalite was formed after 2 days heating in the methylamine medium, no crystalline phase was detected after heating the same gel for 14 days in the presence of TiC14 (TS-I-a). This shows that, as in the case of A13+ ions and Ga 3+ ions [6], the presence of Ti 4+ impedes the growth of MFI framework. The absence of any XRD peaks corresponding to TiO 2 (anatase ...) indicates that the amorphous phase is still composed of stable Ti-Si oligomers. Indeed methylamine and TIC14 admixtures heated under similar conditions without silica, yield pure anatase. The effect of some other potential Ti-complexing agents on the crystallization of titanosilicates was examined. Adding either HC1 or oxalic acid did not improve the crystallization kinetics, the reaction mixtures being still amorphous after 10 days heating (TS-II-a and TS-VI-a). In contrast, the presence of hydrogen fluoride markedly increased the kinetics of crystallization. A highly crystalline (84%) MFI product was obtained after 6 days heating (TSIII). Indeed, fluoride ions are excellent complexing (solubilizing) agents towards silica [ 11 ]. As they also form soluble complexes with titanium ions, it is expected that their adding would increase the solubility of both titanium and silicon species, even at basic pH values achieved in the methylamine medium, and hence improve the crystallization kinetics. The most efficient way to dramatically accelerate the crystallization of titanosilicates was the use of the in situ seeding method (TS-I-b). Compared with classical seeding (dry silicalite added to the final gel prior to heating, TS-I-c), the in situ seeding method proved to be far more efficient: 81% crystalline titanosilicate was obtained after 6 days heating, versus a 50% crystalline phase recovered after 10 days heating in the former case. Homogeneous crystallites were also as rapidly obtained when TIC14 was diluted with either HC1 or oxalic acid solution, before it is added to the preheated silicate gel (TS-II-b and TS-VI-b). 3.2 Crystallization of boro-titanosilicates In the case of titanosilicates synthesized by the conventional method and without using F-ions, the reaction mixture was still amorphous after 14 days heating (TS-I-a). However, upon simultaneous adding of boron and titanium (BTS-I involving 4 B and 4 Ti / 96 T atoms; T=Si+B+Ti), some MFI crystals were detected (34% crystallinity after 14 days heating). As the amount of initial titanium decreased from 4 mole / 96 T to 0 while the boron concentration stayed constant (4 B / 96 T), the crystallization accelerated and a shorter time was required to obtain highly crystalline products (compare BTS-I, BTS-III-a, BTS-IV and BS, Table 1). These findings indicate that the presence of titanium in the initial gel inhibits the crystallization; irrespectively to boron, that accelerates the crystallization. Adding of hydrogen fluoride led to the rapid crystallization of boro-titanosilicate (BTSII) just as in the case of titanosilicate synthesis. The in situ seeding method was also tested in the case of boro-titanosilicates. The preheated borosilicate gel without titanium contained a small amount of borosilicate crystallites (5% crystallinity estimated from n-C6 sorption data). As in the case of titanosilicates, the in situ seeding procedure accelerated the crystallization rate of boro-titanosilicates (compare samples BTS-III-a and BTS-III-b, Table 1).
Table 1 Boro-titanosilicatessynthesized through the methylamine route Samples (code) Silicalite TS-I-a TS-I-b TS-I-c TS-11-a TS-11-b TS-111 TS-IV TS-V TS-VI-a TS-VI-b BS BTS-I BTS-I1 BTS-111-a BTS-111-b BTS-IV
Procedure
Complexing ~el.comu.') agent (z mol) B Ti
conventional
-
conventional in situ seeding conventional (seeds) conventional in situ seeding conventional conventional conventional conventional in situ seeding conventional conventional conventional conventional in situ seeding conventional
-
-
8.0 HCl 8.0 HCl 100 HF 100 HF 100 I-IF 20 ox. acid 20 ox. acid -
50 HF
-
-
-
'
Cry st. time Crystallinity
~roducts'
(days)
(%)
B')
2
100
-
Unit cell
T~(EDx)~)T~(xRD)~)vo~u~~ (A3)
-
-
5339
Amorph. 81 50 Amorph. 57 84 100 88 Amorph. 75 100 34 84 75 96 100
Gel composition: (96-x-y) Si02 - x H3B03 - y T i c 4 - 25 TPABr - 300 MeNH2 - z complexing agent - 3500 H20 1) mole 1 96T atoms (T=Si+B+Ti) 2) by 1 1 NMR ~ 3) by EDX surface analysis 4) calculated from the unit cell volume expansion and taking into account the contraction due to the presence of framework boron
249 SEM images indicated that uniformly and similarly shaped crystallites were obtained, from both the conventional and the in situ seeding method. 3.3 Characterization of titanosilicates IR spectroscopy proved to be an easy tool to characterize titanosilicates. The unique band characteristic of titanosilicates and occurring near 960 cm-1 has been attributed to an asymmetric stretching mode of SiO4 bonded to Ti4+ ions in tetrahedral zeolite sites [ 12]. The titanosilicate TS-III synthesized by the conventional method in the presence of HF showed a distinct IR peak at 960 cm ~ which is not detected in the spectrum of silicalite (Fig. 1). All titanosilicates synthesized by the in situ seeding method also clearly exhibit this band. The unit cell volume variation calculated from the shift of specific XRD lines also gives important information on the possible heteroatom incorporation in the zeolite framework. When a Ti 4+ ion, larger than the substituted S i4§ incorporates the MFI framework, the longer Ti-O bond results in an expansion of the unit cell volume of the titanosilicate with respect to that of silicalite. The unit cell parameters calculated from XRD data for various titanosilicate phases are presented in Table 1. The unit cell volume of silicalite synthesized from the methylamine media is identical to the one characterizing silicalite grown from current media using TPAOH. The unit cell volume of titanosilicates synthesized from gels involving initial Ti / 96 T ratios of 4 and 6 through conventional procedures in the presence of HF (samples TS-III and TS-V) showed a marked increase (about 5370 ,~3) with respect to that of silicalite (5339 A3), while the lattice of the sample TS-IV, involving 2 Ti / 96 T initial ratios is logically slightly less expanded (5362 ~3). The unit cell volume of samples obtained by the in situ seeding method (TS-I-b and TS-VI-b) also showed a similar increase (respectively 5366 and 5361 ,~3) with respect to that of silicalite. These results strongly support the IR data suggesting that titanium ions were indeed incorporated in the framework. A relationship between the unit cell volume of a titanosilicate and the quantity of lattice Ti has been proposed [12]. Using this correlation, we could evaluate the amount of lattice titanium in the different titanosilicate phases obtained by using the methylamine route. The incorporation extends to about 1.7 Ti / 96 T for initial ratios of 4 Ti / 96 T, thus smaller than the amount measured in crystals grown from conventional media involving Ti and Si alkoxides and TPAOH (about 2.5 Ti / 96 T, as reported in the original patent [13]). Sample TS-III (titanosilicate synthesized in the presence of HF by the conventional method) showed a neat UV band at about 230 nm, corresponding to isolated framework titanium ions involving a tetrahedral coordination [ 14]. This constitutes a further evidence of the existence of framework titanium ions. The sample synthesized from gels involving initial 6 Ti / 96 T ratios (TS-V) exhibits, along with this UV band, an additional very weak shoulder at 320 nm which was not detected in samples TS-III and TS-IV (respectively involving initial ratios of 4 Ti / 96 T and 2 Ti / 96 T). This broad band has been attributed to octahedrally coordinated Ti in anatase [14]. These findings indicate that a too large amount of titanium (more than 4 mole / 96 T ) in the initial gel leads to the formation of anatase as side phase, in quantities too small to be detected by XRD. 3.4 Characterization of boro-titanosilicates l lB-NMR has been shown to be the key technique to determine the quantity and the coordination of boron in various borosilicate [10,15] and boro-titanosilicate [4] zeolites. All MFI-borosilicates [16] and boro-titanosilicates (BS and BTS samples, Table 1) synthesized in the presence of methylamine showed only one narrow peak at -3.6 ppm which was assigned to framework tetrahedral BO 4 units. No peaks occurring at +6 ppm (trigonal boron) and at-2 ppm (tetrahedrally coordinated boron in amorphous phase) were detected, confirming the efficiency of the methylamine route in incorporating boron in the T sites of the MFI structure, sole or in the presence of titanium.
250 The amount of boron in as-synthesized I crystallites was calculated from llB-NMR line intensities using the appropriate calibration curves [ 10,15] and the results are reported in Table 1. Trong On et al. [3] reported that boro-titanosilicates synthesized in the presence of TPAOH and H202 contained almost the same amount of boron as the corresponding Ti-free borosilicates: they coneluded that the quantity of titanium in the initial gel did not affect the amount of framework boron under l I I ' I I i their synthesis conditions. In contrast, the boron 1400 1200 1000 800 600 400 content in our boro-titanosilicate phases varied with Wave number (cm- 1) the initial quantity of titanium. The amount of Fig. 1 IR spectra of zeolites synthesized 2.72 mole B per unit cell from methylamine media decreased to 1.86 mole (a) TS-III: titanosilicate (conventional synthesis) when titanium ions (1 Ti / (b) TS-I-b: titanosilicate (in situ seeding) 96 T) were added in the (c) BTS-II: boro-titanosilicate initial gel (sample BTS-IV) (d) BS: borosilicate and a further increase of the titanium content up to 4 mole/96 T led to a further slight decrease of the boron amount (sample BS, to be compared to BTS-IV, BTS-III-a and BTS-I). These findings support the assumption that methylamine forms complexes with both Ti and B species while it also solubilizes the various Si species by bringing the pH to basic values. The stability of these complexes could be mutually affected by assuming that the presence of titanium ions in the system prevents to some extent the formation of the adequate boronmethylamine complexes, and vice-versa, at least at certain stages of the crystallization process (see below). The IR spectra of several metallosilicates are shown in Figure 1. All samples show the IR bands at 455, 800 and 1100 crn- that typically characterize the vibration of the SiO 4 tetrahedra in the MFI framework, as well as the band at 555 cm-1 which corresponds to the vibration of five membered rings in the pentasil structure. In addition to these bands, the borosilicate shows a shoulder peak at 920 cm -I and very week band at 1380 cm ~. The IR band at 920 cm 1 has been assigned to tetrahedrally coordinated framework boron, while the one at 1380 cm -~was found to correspond to trigonal boron species [ 17]. As described above, the titanosilicate samples as well as the BTS-II sample showed a quite well resolved band at 960 cm 1 which is generated by the presence of the lattice titanium. The combination of 11B-NMR and IR data confirms the simultaneous presence of Ti and B in the framework of boro-titanosilicate crystals. The framework titanium content in the bulk of the boro-titanosilicates could be approximately estimated from the unit cell volumes calculated from XRD data, taking into Ca)
/'x
251 account the lattice contraction caused by the presence of boron; the concentration of which was evaluated by NMR (Table 1). The maximum framework Ti concentration as evaluated by XRD does not exceed 0.7 mole / 96 T. All the values are actually slightly lower than those found in the corresponding titanosilicates: 1.3 to 1.6 mole / 96 T, suggesting that the presence of boron also hinders the incorporation of titanium into MFI frameworks. Spot EDX measurements of the Ti concentrations in individual crystallites also indicate that boro-titanosilicates contained less titanium than the corresponding titanosilicates. On the other hand, the higher EDX values with respect to the global bulk Ti concentrations evaluated by XRD could indicate that the surface of the boro-titanosilicate samples is slightly enriched in Ti with respect to their core. Indeed, in the case of large crystals, the EDX technique would probe elemental concentrations more readily in their outer shell region than in their core [6, 18]. These findings suggest that the hindering of Ti incorporation by the presence of boron is apparent and essentially occurs in the beginning of the crystal growth process, when boron is more readily incorporated in the framework than Ti, possibly in relation to the different complexation power of both metals with methylamine or HF. By contrast, similar EDX and XRD values suggest that the corresponding titanosilicates involve a less pronounced Ti gradient throughout the crystallites when they are crystallized in the presence of both methylamine and HF mineralizing species (samples TS-III, -IV and-V). Moreover, titanosilicates involve a quasi homogeneous Ti framework distribution when methylamine is the only mobilizing species used (sample TS I-b), as already observed for A1- and Ga-MFI [6]. The gradient concentration of Ti in large crystals grown in the presence of various mineralizing-complexing agents is now being investigated by combining XPS data with other depth profiling evaluation techniques [19]. Finally, while all the titano- and boro-titanosilicates samples showed the typical UV band at about 230 nm corresponding to isolated framework titanium ions in tetrahedral coordination, all the boro-titanosilicate samples exhibited a very weak additional shoulder which was attributed to anatase impurities. This could confirm that the addition of boron in the initial gel first leads to the easy formation of a borosilicate (Ti poor) framework (core of the final crystal) and that more Ti is preferentially incorporated during a later stage of the growth process when the gel is somewhat depleted in boron, resulting in a Ti enriched outer rim. This situation would result in an overall restricted Ti incorporation in the zeolite so that any excess of Ti would incorporate in the other Ti species currently stable under mild hydrothermal conditions, such as anatase. 4. C O N C L U S I O N Pure MFI type titanosilicates and boro-titanosilicates were synthesized rapidly and in good yield by using the new procedure involving alkali free alkylamine (optionally admixed with HF) as mobilizing agent, and TPABr. Silica and titanium tetrachloride were used as Si and Ti sources respectively. One of the advantages of this new procedure compared to conventional methods leading to fitanosilicates, is that highly crystalline titanosilicates can be obtained without the use of costly TPAOH or Si and Ti alkoxides. The presence of titanium in the methylamine bearing gel slows down the crystallization of Ti-MFI. Its crystallization could be dramatically increased by a further addition of F ions. Compared with titanosilicates, boro-titanosilicates crystallize fairly rapidly in methylamine media. The in situ seeding method (addition of titanium reactants into a preheated silicate or borosilicate gel) markedly accelerated the crystallization of both fitanosilicates and borotitanosilicates, the obtained crystals still exhibiting a uniform shape and size. IR data, the lattice volume expansion (XRD) and UV-vis spectroscopy confirmed the incorporation of titanium into the MFI framework of titanosilicates or boro-titanosilicates grown by using either the conventional or the in situ seeding methods, llB-NMR confirmed the presence of framework boron along with titanium in the framework of boro-titanosilicates. The
252 amount of boron in boro-titanosilicates is lower than in the corresponding borosilicates. The relative hindering of Ti incorporation by the presence of boron and vice-versa was interpreted by considering the preferential incorporation of boron in the beginning of the growth process allowing an easier further Ti incorporation at the end of the crystallization. These somewhat sequential incorporation may be related to the different strength of the corresponding metallic complexes with HF and/or methylamine. This can also explain the formation of traces of extra framework Ti species (anatase) during the last stages of the growth. REFERENCES
10 11 12 13 14 15 16 17 18 19
M.G. Clerici and. P.J. Ingulina, J. Catal. 140 (1993), 71 J.S. Reddy, R. Kumar and S.M. Csicsery, J. Catal., 145 (1994), 73 D. Trong On, S. Kaliaguine and L. Bonneviot, J. Catal.,157 (1995), 235 D. Trong On, M.P. Kapoor, S. Kaliaguine, L. Bonneviot and Z. Gabelica, Stud. Surf. Sci. Catal., 97, (1995), 535 Z. Gabelica, R.J. Monque and G.P. Giannetto, US Patent N ~ 5 354 719 (1994) Z. Gabelica, G. Giannetto, F. Dos Santos, R, Monque and R. Galiasso, in "Proc. 9th Intern. Zeolite Conf., Montreal, 1992, R. Von Ballmoos et al., Eds,Butterworth- Heinemann, New York, 1993, Vol. I, pp 231 Z. Gabelica, M. Wiame, J. G6rard and M. Shibata, submitted for publication M. Shibata, J. G6rard, T. Inui and Z. Gabelica, submitted for publication Z. Gabelica, J. B.Nagy, E.G. Derouane and J.P. Gilson, Clay Minerals, 19 (1984), 803 Z. Gabelica, J. B.Nagy and G. Debras, Stud. Surf. Sci. Catal., 19, (1984), 113 H. Kessler, J.M. Chezeau, J.L. Guth, H. Strub and G. Coudurier, Zeolites, 7, (1987), 360 M. R. Boccuti, K. M. Rao, A. Zecchina, G. Leofanti, and G. Petrini, Stud. Surf. Sci. Catal., 48, (1989), 133 M. Taramasso, G. Perego and B. Notari, US Patent N ~ 4 410 501 (1983). A. Zecchina, G. Spoto, S. Bordiga, A. Ferrero, G. Petrini, G. Leofanti, and M. Padovan, Stud. Surf. Sci. Catal., 69, (1991), 251 Z. Gabelica, J. B.Nagy, P. Bodart and G. Debras, Chem. Letters, 1984, 1059 Z. Gabelica and M. Shibata, submitted for publication R. de Ruiter, J.P.M. Kentgens, J. Grootendorst, J.C. Jansen, and H. Van Bekkum, Zeolites, 13, 128 (1993). Z. Gabelica, N. Blom and E.G. Derouane, Appl. Catal., 5, (1983), 227 M. Shibata, Ph.D. Thesis, in preparation
H. Chon, S.-K. lhm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials
Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
253
Synthesis, characterization and c a t a l y t i c p r o p e r t i e s of vanadium containing VPI-5 Karuna Chaudhari, Tapan Kr. Das, A.J. Chandwadkar, J.G. Chandwadkar" and S. Sivasanker* National Chemical Laboratory, Pune 411 008, India 'Chemistry Department, University of Poona, Pune 411 007, India A novel vanadium containing molecular sieve with VPI-5 structure has been synthesized XRD, UV-vis, ESR, NMR and sorption studies suggest that the vanadium ions are in the framework positions. V-VPI-5 is found to be active in the catalytic oxidation of large organic molecules such as 2-methyl naphthalene in the presence of both organic peroxides and 1-1202. 1. INTRODUCTION A number of vanadium containing molecular sieves possessing selective oxidation properties have been reported so far. However, the application of these molecular sieves as catalysts is limited as all the materials, except the mesoporous vanadosilicate, V-MCM-41, catalyse the oxidation of only small molecules. VPI-5 is a large pore aluminophosphate molecular sieve with pores made up of 18-membered tings and having a diameter of-- 1.2 nm [1]. We now report the synthesis, characterization and catalytic properties of vanadium containing VPI-5. The physico-chemical characterization of the samples reveals the presence of V ions in the lattice. Besides the material is found to catalyse the selective oxidation of the large molecule, 2-methyl naphthalene in the presence of both organic peroxides and 1-1202. 2. EXPERIMENTAL The synthesis of V-VPI-5 was carried out hydrothermally using psuedoboehmite (CatapalB, 73% A1203, Vista Chemicals), vanadyl sulphate trihydrate (Aldrich, 99.99%), phosphoric acid (S.D. fine chemicals, 85% solution) and tetrabutyl ammonium hydroxide. The composition of the gel in terms of moles of oxides was Al203 " P205 "x VO2" TBAOH 950 H20 ; x < 0.04. In a typical s3nlthesis, pseudoboehmite (4.2 g, Catapal-B) was mixed with water (8.0 g). A diluted solution of orthophosphoric acid (85%; 6.93 g) in water (3 g) was added slowly with stirring to the alumina slurry. Vanadyl sulphate trihydrate (0.521 g) dissolved in water (2.0 g) was then added to the above AIPO4 gel and aged at 298K for 24 hours. Then, tetrabutyl ammonium hydroxide (19.46 g; Aldrich, 40 wt.% solution) was added to the aged gel and stirred for one hour. The gel was transferred to a stainless steel autoclave and allowed to crystallize at 418K for 24 hours. The crystalline material thus obtained was washed with hot water to remove occluded templates. The sample was dried at room temperature. The sample was treated with NH4OAc to remove surface vanadium present [2]. It was then treated two times with dilute H202 (1"10, wt.) to convert the V4§ to V s+ , washed with water and dehydrated slowly at 623K in high vacuum overnight. For comparison purposes, a sample
254 of VPI-5 was synthesized following the procedure reported earlier [3]. The as-synthesized, dried and oxidized samples were examined for phase purity by XRD, morphology by SEM and the state of vanadium by UV-vis, NMR and ESR spectroscopies. The V4+ and V 5+ contents in the as-synthesized, NI-I~OAc washed and H202 treated samples were estimated by chemical analysis: atomic absorption spectroscopy, inductively coupled plasma analysis and permanganometric titrations [4] (Table 1). Adsorption of water, n-hexane and tri-isopropyl benzene was carried out to ascertain void volumes. The catalytic reactions were carried out in a batch (100 ml) reactor in organic solvents or in aqueous medium at 353K. 3. RESULTS AND DISCUSSION
3.1 Chemical composition The four V containing VPI-5 samples were prepared with different V (as V4§ inputs in the gel (Table 1). The percentage incorporation of vanadium in the crystalline material increased with decrease in V-content in the gel. On extraction with NH4OAc (1 M solution), a small quantity of extralattice V (mostly V4+) was removed from all the samples. In the case of the sample with the least vanadium content (V-VPI-5(1)), only 3% of the vanadium ions was extracted, while a much larger and nearly constant amount of --11-13% vanadium was extracted from the other (V-rich) samples. After H202 treatment only V 5§ was present in the samples. Table 1 Chemical composition of V-VPI-5 samples. Composition (atom ratio); A I : P : V( %V4+, %V5+)'
Sample Synthesis gel
As-synthesized
NH4OAc treated
H202 treated
V-VPI-5(1)
1:1:0.0033
1:0.98:0.0032(92,8)
1:0.98:0.0031(83,17)
1:0.98:0.0031
V-VPI-5(2)
1:1:0.0100
1:0.97:0.0084(81,19)
1:0.97:0.0075(70,30)
1:0.97:0.0075
V-VPI-5(3)
1:1:0.0200
1:0.96:0.0140(76,24)
1:0.96:0.0123(66,34)
1:0.96:0.0123
V-VPI-5(4)
1:1:0.0400
1:0.98:0.0160(71,29)
1:0.98:0.0140(62,38)
1:0.98:0.0140
'The numbers in brackets refer to the % of V4+ and V 5§ in the samples.
3.2 X-ray diffraction The XRD patterns of the VPI-5 and the V-VPI-5 samples are presented in Figure 1. They are all similar and do not reveal the presence of impurity phases. Since V4+ and V 5+ are larger than AI3+ and pS+ (ionic radii : V4+(CN = V), 0.053; Vs+(IV), 0.036; AIa+(IV), 0.039 and Ps§ 0.017 nm), their incorporation in the lattice of the VPI-5 is expected to increase its unit cell size [5,6]. We do observe a systematic increase in the d-values of all the lines in the XKD patterns, on incorporation of vanadium in VPI-5. For example, in the case of the typical line at 20 -- 5.38 ~ the d-value increases from 1.6412 nm (VPI-5, pattern A in Figure 1) to 1.6536, 1.666, 1.6695 and 1.6723 nm (V-VPI-5, patterns B, C, D and E respectively in Figure
255 1). The above results suggest that V ions are probably incorporated in the framework in the samples. It is likely that the vanadium ions are replacing both AI3+ and pS+. The V4§ ions probably replace both AI3+ and pS+, the V 5+ ions replacing preferentially the pS+ ions. However, in view of the much larger radii of the V 4§ and V s§ ions (compared to the AI3+ and P~+ ions), the isomorphous replacement is like to lead to defect sites in the framework as has already been reported by earlier workers in the case ofvanadosilicates [7]. The crystallinity of all these samples remained the same even on vacuum dehydration. 3.3 SEM The SEM pictures do not reveal noticeable differences in morphology between V free and V containing samples. The crystals are seen as long needles (10-60 ~tm) arranged in a definite manner to produce agglomerates of 300 to 500 l.tm diameter, the entire structure suggesting growth from the center to the outer surface of the agglomerates (Figure 2).
I0
20
30
40
20---=-
Figure 1. XRD patterns of as-synthesized samples. A:VPI-5, B:V-VPI-5(1), C:VVPI-5(2), D:V-VPI-5(3), and E:V-VPI5(4).
Figure 2. SEM picture of as-synthesized V-VPI-5(3).
256 3.4 UV-vis
The UV-vis reflectance spectra of the as-synthesized and H202 treated samples revealed a band around 320 nm in both the samples. This band has been suggested to be due to low energy charge transfer (LCT) between oxygen and V 5+ ions present in tetrahedral environments [2,8]. The intensity of the band did not decrease on extraction of the samples with NH4OAc suggesting that the V s+ species are strongly held in the samples and are probably present in the framework positions. The intensity of the 320 nm band increases on treatment of the sample with H202 due to an increase in V 5+ions in the samples. 3.5 ESR
All the as-synthesized vanadium samples exhibit sharp 8-line ESR spectra at room temperature. A representative spectrum of V-VPI-5(3) (Figure 3) reveals spectral parameters of g l l - 1.907, gL = 1.966, All - 204.28G and A• = 75G suggesting that V4+ ions are present in square pyramidal or distorted octahedral symmetries [9]. Sharma et aL [10] have shown that the magnitude of the quantity B (= Agj}/AgL) can be used to decide whether the species is in a distorted octahedral or a square pyramidal symmetry, values closer to 1 signifying nearly octahedral symmetry. The value of 2.6 obtained in our case suggests that the species are probably in a distorted octahedral symmetry. The intensity of the spectral lines decreases slightly on extraction with NH4OAc (Figure 3, spectrum B). The ESR parameters of the assynthesized sample (A) and the NH4OAc-extracted sample both after gentle drying at 300K and after calcination at 623K (sample B) were nearly identical.
C
2000
Figure 3. ESR spectra of V-VPI-5(4). A:as-synthesized, B:NH4OAc treated and C:H202 treated and dehydrated.
0
- 2 0 0 0 -~)(X) PPld
Figure 4. 51V NMPx spectra of oxidized and dehydrated samples. A:V-VPI-5(1), B:V-VPI-5(2) and V-VPI-5(3).
257 As the ESR spectra are attributable to distorted Oh species, it appears likely that the vanadium ions are attached to the framework at defect sites with partial framework connectivities, the additional ligands necessary for Oh co-ordination probably being tightly held water molecules. The samples lost ESR activity on oxidation with H202 and dehydration at 623K in vacuum (Figure 3, spectrum C). 3.6 NMR StV spectra of the oxidized and dehydrated V-VPI-5(1), V-VPI-5(2) and V-VPI-5(3) samples were recorded under static conditions using a Bruker MSL300 spectrometer (Figure 4). All these samples exhibit a single broad signal centred at 8 = -600 + 50 ppm (Figure 4). The near isotropic nature of the signals and their positions around -600 ppm suggest that these are probably due to Q0 species present in nearly regular tetrahedral positions and associated with O-ions [11,12].
It is likely that the V4§ions present in the octahedral symmetry (I; shown below) in the assynthesized sample transform into tetrahedral V s§ species (II) through oxidation and loss of H20 ligands during H202 treatment and evacuation. The absence of a signal at 8 = - 3 l0 ppm suggests that V2Os-like phases are not present in the samples.
H
H
~AI~o 0 O~V4~'OH HO~AI~ ,, OXIDN.--- ~ V HO--At -H20 / 7 0 / ' ! ~ O x AI 70 O~ 9jAI H/O\H ~ AI AI -qAk
x? /
4. SORPTION STUDIES Sorption measurements of water, n-hexane and tri-isopropylbenzene by VPI-5 and VVPI-5 samples were obtained at 298K ( P/po = 0.5) using a McBain-Baker type gravimetric unit having a calibrated silica spring. The sorption values obtained for VPI-5 are 30.9%, 17.3% and 9.4% for water, n-hexane and tri-isopropylbenzene, respectively. On incorporation of V (e.g. sample V-VPI-5(3)), these values were 31.53%, 17.8% and 9.8%, respectively. The similarity in values suggests that the incorporation of vanadium did not lead to blockage of the pores. In fact, the small increase in sorption by the V-VPI-5 sample probably suggests an increase in void volume clue to expansion of the lattice by the V-ions.
258 5. CATALYTIC ACTIVITIES The results of the hydroxylation of phenol with H202 and the oxidation of 2-methyl naphthalene with H202 and tertiary butylhydroperoxide (TBHP) over V-VPI-5 samples are presented in tables 2 and 3, respectively. Table 2 Activity of the samples in the hydroxylation of phenol' Sample
Conv. (mol.%)
H202 Select.(mol%)
Product distribution (wt.%) BQb
CATb
HQ b
V-VPI- 5( 1)
12.81
38.5
29.70
68.7
1.60
V-VPI-5(2)
14.88
44.7
24.60
67.3
8.10
V-VPI-5(3)
16.35
49.1
23.50
68.2
8.30
V-VPI-5(4)
18.10
54.3
15.28
70.6
14.12
V-VPI-5(4) NH4OAc treated
17.90
52.6
16.30
69.8
13.90
V-impregnated VPI-5 (2% V205)
1.00
3.9
50.00
25.0
25.00
'Reaction conditions : Catalyst = 100 mg, Solvent(water) = 10 g, Phenol/H202(mole) = 3, Temp. = 353K, Reaction time = 24 h, Substrate = lg. bBQ, benzoquinone; CAT, catechol; HQ, hydroquinone. The catalytic activity tests were carried out using H202 treated samples with and without NH4OAc treatment. Both the samples exhibited almost the same catalytic activities (Table 2). As some amount of vanadium was extracted by NH4OAc, it appears that only non-extractable vanadium (V in the framework) has been catalytically active. In general, in the case of both phenol hydroxylation and oxidation of 2-methyl naphthalene, the activities and peroxide selectivities increase with increase in V-content of the samples. This is similar to earlier reports over titano and vanadosilicates [ 13,14]. The hydroxylation of phenol produces more benzoquinone than generally reported over titanosilicates [13]. Such an overoxidation has already been reported in the case of the vanadosilicate, VS-2 [5]. Again, the oxidation of 2-methyl naphthalene produces more side chain oxidation products than ring hydroxylation products. Such a selectivity for side chain oxidation products has also been reported in the case of VS-2 during the oxidation of toluene [5]. The V-impregnated VPI-5 samples are found to possess very little activity confirming that the activity of V-VPI-5 samples arises from V-ions incorporated in the framework.
259 Table 3 Oxidation of 2-methyl naphthalene over V-VPI-5" Sample
Conv. (mol.%)
Product distribution (wt.%)
TBHP select. (mol.%)
2-naphthaldehyde
2-naphthalene methanol
Others b
V-VPI-5(1)
5.7
18.80
80.7
12.3
7.0
V-VPI-5(2)
6.8
21.63
75.0
16.1
8.9
V-VPI-5(3)
8.1
25.40
72.8
16.0
11.2
V-VPI-5(4)
9.7
30.00
70.1
18.5
11.4
V-VPI-5(4) c
8.6
26.60
71.2
17.5
11.3
V2Os(2%) impregnated VPI-5 "Reaction conditions" Catalyst = 100 mg, Solvent(acetonitrile) = 10 g, Substrate/TBHP(mole) = 2, Temp. = 353K, Reaction time = 24 h, Substrate = lg. bMostly ring hydroxylation products. cHzOz used as oxidant; reaction conditions same as in the case of TBHP runs except, substrate~zOz (mole) = 2. In general, medium pore vanado and titanosilicates such as VS-1 or TS-1 can not oxidize molecules such as 2-methyl naphthalene due to pore size restrictions. Besides,. they can not utilize TBHP as an oxidant due to its large size and spatial restrictions inside the pores. VVPI-5 is able to not only oxidize the large molecule, 2-methyl naphthalene, it is also able to use TBHP as the oxidant. As the impregnated VPI-5 samples do not possess any activity, the activity of the V-VPI-5 samples is due to the V-ions in the framework and inside the pore system. Thus, V-VPI-5 appears to be a good large-pore selective oxidation catalyst. 6. CONCLUSIONS Highly crystalline V-containing VPI-5 samples have been synthesized. These samples contain both V 4§ and V s§ mainly in framework positions. The small amount of non-framework ions (mostly V 4+) is easily removed by washing with an NH4OAc solution. While direct evidence for V-incorporation in the framework is obtained from XRD data, the ESR, UV-vis and NMR studies also suggest such incorporation. The V-VPI-5 samples are catalytically active in the hydroxylation of phenol and the oxidation of 2-methyl naphthalene.
260 ACKNOWLEDGMENTS We thank Dr. D. Chakrabarty for ICP analysis. TKD thanks CSIR for a research fellowship. SS thanks IFCPAR, New Delhi for partial funding. REFERENCES
.
9. 10. 11. 12. 13. 14.
M. Davis, C. Saldarriga, C. Montes, J. Garc~s aM C. Crowder, Nature, 331 (1988) 698. G. Centi, S. Perathoner, F. Trifiro, A.. Aboukasis, C.F. Aissi and M. Guelton., J. Phys. Chem., 96 (1992) 2617. M.E. Davis and D. Young, Stud. Surf. Sci. Catal., 60 (1991) 53. I.M. Kolthoff, Treatise on Analytical Chemistry, Interscience, New York, Part II, 8 (1963) 226,260. P.R.H.P. Rao, A.V. Ramaswamy and P. Ratnasamy., J. Catal., 137 (1992) 225. A. Tuel and Y. Ben Taarit, Appl. Catal., A 102 (1993) 201. T. Sen, V. Ramaswamy, S. Ganapathy, P.R. Rajamohanan and S. Sivasanker, J. Phys. Chem. (in press). A. Corma, J.M. Lopez Nieto and N. Parades, Appl. Catal., 104 (1993) 161. A. Davidson and M. Che, J. Phys. Chem., 96 (1992) 9909. V.K. Sharma, A. Wokaun and A. Baikar, J. Phys. Chem., 90 (1996) 2715. O.B. Lapina, V.M. Mastikhin, A..A.. Shubin, V.N. Krasilnikov and K.I. Zamaraev, Progress in NMR Spectroscopy, 24 (1992) 457. I. Moudrakovski, A. Sayari, C.I. Ratchffe, J.A. Ripmeester, K.F. Preston, J. Phys. Chem., 98 (1994) 10895. A. Thangaraj, R. Kumar and P. Ratnasamy, J. Catal., 131 (1991) 294. P.R.H. Rao and A.V. Ramaswamy, Appl. Catal. A, General, 93 (1993) 123.
H. Chon, S.-K. Ihm and Y.S. Uh (Editors) Progress in Zeolite and Microporous Materials Studies in Surface Science and Catalysis, Vol. 105 9 1997 Elsevier Science B.V. All rights reserved.
261
Crystallization of Titanium Silicalite-1 from Gels Containing Hexanediamine and Tetrapropylammonium Bromide A. Tuel Institut de Recherches sur la Catalyse. C.N.R.S. 2, av. A. Einstein 69626 Villeurbanne Cedex FRANCE
Abstract
Titanium substituted silicalite-1 (TS-1) samples have been synthesized using hexanediamine (C6DN) and tetrapropylammonium bromide (TPABr). Following this method, titanium could be incorporated up to a level of about 2 Ti/unit cell in the framework of silicalite-1. Crystals had a typical habit, very different from those obtained with standard syntheses, which led to exceptionnally high para/ortho ratios in the hydroxylation of phenol with hydrogen peroxide.
1. I N T R O D U C T I O N Usually, the titanium containing silicalite-1 (TS-1) is synthesized using tetrapropylammonium hydroxide (TPAOH) solutions, which provides both the templating molecule and the alkalinity necessary for the crystallization of the zeolite [1]. However, the synthesis requires severe conditions, particularly regarding the presence of alkali cations in the precursor gel [2]. Therefore, TS-1 is a quite expensive catalyst whose synthesis requires the preparation of alkali-free TPAOH solutions. Thus, it would be of great interest to synthesize TS-1 with TPABr as templating molecule as the latter is less expensive than TPAOH and usually free from alkali cations, in contrast to most of the commercial TPAOH solutions. Several authors have shown that pure silicalite-1 could be obtained from gels containing TPABr and an organic (or inorganic) base like piperazine or NH4OH [3,4]. However, crystals were usually very large and syntheses were complicated by the high volatility of NH4OH solutions. Because of the large crystals thus obtained, it was not conceivable to obtain Ti-containing silicalite-1 active in oxidation reactions in the liquid phase following these methods.
262 In the present paper, we report on the synthesis of TS-1 using TPABr as templating agent and hexanediamine (C6DN) as only base. The system was particularly interesting as C6DN has also been reported to direct zeolite structures in the absence of quaternary ammonium cations [5]. We have explored the possibilities of synthesizing TS1 by varying synthesis parameters such as the Ti content, the nature of the silica source or the crystallization conditions. Catalytic performance of such materials in the hydroxylation of phenol is reported and compared with that of a conventional TS-1 sample prepared with TPAOH.
2. E X P E R I M E N T A L TS-1 was synthesized in the following manner: 1.75 g of C6DN was first dissolved in 40 ml of distilled water before the addition of 3 g of silica A 200 (Degussa). Then 0.17 ml of tetrabutyl orthotitanate in 10 ml dry isopropyl alcohol was added and the resulting mixture stirred for about 30 min. Finally, 1.33 g TPABr in 25 ml of distilled water was added and the gel heated at 80~ for 3 h to remove isopropyl alcohol. The gel, whose composition was the following" SiO 2 - 0.01TiO 2 - 0.3C6DN - 0.1TPABr - 50H20 was transferred into a stainless steel teflon-lined autoclave and crystallized at 180~ for 5 days under stirring (250 rpm). The solid was then recovered, washed with distilled water and dried at 120~ in an oven. Occluded organics were removed by calcination of the sample in air at 530~ for 10 h. For comparison a TS-1 sample was prepared with TPAOH using a patent recipe [1] and contained 0.92 wt % Ti. Samples were characterized using conventional methods. X-ray powder patterns were recorded on a Philips PW 1710 diffractometer using the CuKa radiation. U.v-vis spectra were collected on a Perkin Elmer Lambda 9 spectrometer. I.r. spectra were obtained on a Perkin Elmer 580 spectrometer using KBr wafers (1 wt % zeolite). 13C Solid state n.m.r, spectra were recorded on a Bruker MSL 300 spectrometer using a 1H13C CP/MAS sequence with 2 ms contact time and 10 s delay. SEM pictures were collected on a Jeol microscope. Chemical analyses were obtained by atomic absorption after solubilization of the samples in HF-HCI solutions. The hydroxylation of phenol was carried out batchwise following a method previously described [6].
263 3. RESULTS AND DISCUSSION The X-ray powder pattern of as-synthesized sample (corresponding to the gel composition given in the experimental section) shows all the reflections characteristic of the MFI structure but reveals important differences in peak intensities, particularly those corresponding to (0k0) reflections as compared to a conventional TS-1. The systematic increase in (0k0) reflection intensities probably indicates the presence of preferential planes in the crystals. Indeed, crystals are in the form of elongated prisms of about 7 x 2.5 x 0.5 /~m (Fig: 1), a very unusual habit for TS-1 whose particles are generally very small and round-shaped.
(c)
IL--
Fig. 1. SEM pictures of sample 1 (Si/Ti = 76) (a), sample 3 (Si/Ti - 31) (b) and corresponding axes (c) The well developed (ac) planes are thus responsible for the intense (0k0) reflections in the X-ray pattern. As expected, 13C NMR spectrum of the as-synthesized sample shows that only TPA + cations are occluded in the zeolite pores. I.r. spectrum of calcined sample shows an absorption band at 960 cm "1, absent from the spectrum of the pure silica material, and characteristic of metal-substituted zeolites. The optical density of this line, 1960/1800, increases with the Ti content in the samples (Fig. 2). Moreover, the i.r. absorption band at 550 cm "1, due to the presence of double rings in the structure, is
264 clearly splitted, giving a band at 540 cm -1 more intense than that at 560 cm "1. As for Xray reflection intensities, this was attributed to the typical morphology of the crystals obtained by the present synthesis route.
u.c. (A3)
1960/1800 2.0
5380
o~~ ~
~~
5360
1.5
D
5340 _ o
o.6
o.b2
Ti/(Si+Ti)
o.6a
0
0.04
Fig. 2. Evoultion of the u.c. volume and of the optical density of the i.r. band at 960 cm -1 with the Ti content. 3.1. I n f l u e n c e o f t h e t i t a n i u m c o n t e n t
We have synthesized a series of samples by varying the amount of titanium in the synthesis gel. The chemical composition as well as the characteristics of the various samples are listed in Table 1. Table 1 Characteristics of the samples prepared with various Ti contents Si/Ti Sample
Gel
Zeolite
u.c. (~3)
1
100
76
5367 _+ 2
2 3 4
50 33 25
43 31 24
5384 _ 2 5387 _+ 2 5390 _+ 2
265 The unit cell volume increases linearly with the titanium content in the samples up to about 2 wt % Ti. Then, a deviation is observed for higher values, suggesting that samples do not contain only tetrahedrally coordinated titanium species (Fig. 2). Indeed, the presence of extraframework titanium in the samples prepared with low Si/Ti ratios was confirmed by u.v-vis spectroscopy. In contrast to samples 1 and 2 for which the spectrum was composed of a single absorption band at 210 nm, sample 3 shows an additional shoulder at 280 nm, resulting from partially condensed hexacoordinated titanium species [7]. However, we never observed a dinstinct band at 330 cm -1 characteristic of TiO 2. SEM pictures of the various samples show a change in the crystal habit and size with Ti incorporation (Fig. 1). Starting from about 0.1-0.2 for sample 1, the a/c ratio increases to 0.65 for sample 3. In the same time, the thickness (along the b-axis) increases with the Ti content from 0.3-0.4 ~tm for silicalite-1 to 1.5/~m for sample 3. The change in crystal habit has an influence on X-ray diffraction intensities and the relative intensities of the i.r. bands at 540 and 560 cm -1. For sample 3, both X-ray powder pattern and i.r. spectrum are very similar to those of a conventional TS-1 synthesized with TPAOH. 3.2. Effect of the diamine concentration Samples have been prepared with Si/Ti = 100 in the gel and varying the
C6DN/SiO 2 ratio from 0.075 to 1.2. As a general trend, this ratio has not a great influence on the composition of the TS-1 obtained (Table 2). However, as for the titanium content, increasing the amount of C6DN in the precursor gel changes the crystal morphology, from elongated to cubic-like particles. As an example, crystals of sample 9 prepared with C6DN/SiO 2 = 1.2 are very similar to those of sample 3 obtained with C6DN/SiO 2 = 0.3 but Si/Ti = 33 (see Fig. 1). Table 2 Characteristics of the samples synthesized with various amounts of hexanediamine Si/Ti Sample 5 6 7 8 9
C6DN/SiO 2 0.075 0.15 0.3 0.6 1.2
'
Gel
Zeolite
100 100 100 100 100
77 86 76 89 78
u.c. (/~3) 5349 5362 5367 5363 5365
_+ 2 +_ 2 _ 2 _+ 2 +_ 2
266 3.3. Influence of the TPABr concentration
Assuming 4 TPA + cations per unit cell of TS-1, the minimum amount required to fully crystallize TS-1 corresponds to TPA/SiO 2 = 0.042 in the gel. For lower values, there could be a competition between TPA + and hexanediamine to direct the MFI and ZSM-48 structures, respectively. However, it has been shown that addition of TPABr in a pure silica gel containing C6DN strongly favoured the formation of silicalite-1 with respect to ZSM-48, even for TPA/SiO 2 ratios as low as 0.025 [5]. We have performed a series of syntheses for which the TPA/SiO 2 ratio was varied from 0 to 0.1. For TPA/SiO 2 ratios > 0.045, highly crystalline TS-1 is obtained. For lower ratios, TS-1 is obtained together with amorphous material but Ti-ZSM-48 is never observed, suggesting that this zeolite can probably not be obtained under the present synthesis conditions. The amount of TS-1 in the batch, estimated from the intensity of the (501) reflection in the X-ray pattern, increases linearly with the TPA/SiO 2 ratio (Fig. 3).
100
I TS-1 Yield (%)
oj,,,.~,..~~
o
8O 6O 4O 2O O0
TPA/SiO2 !
0.025
I
0.050
!
0.075
0.1
,...._
Fig. 3. Percentage of TS-1 in the batch as a function of the TPA/SiO 2 ratio 3.4. Influence of the silica source
In conventional syntheses, the nature of the silica source greatly influences the morphology of TS-1 crystals and the Ti incorporation. In the present case, syntheses performed with tetraethyl orthosilicate or colloidal silica Ludox AS-40 led to TS-1 crystals very similar to those obtained with A 200, indicating that the nature of the silica
267 source was not as critical as for syntheses performed with TPAOH [8]. Moreover, the Ti content was approximately the same in all samples.
3.5. Catalysis Among all the reactions catalyzed by TS-1, the hydroxylation of phenol is of particular interest as it permits to obtain para and ortho dihydroxybenzenes with an excess in the para isomer. However, Van der Pol et al. [9] have reported that the crystal size strongly influences the performance of the catalyst and that good activities can only be obtained with TS-1 crystals smaller than 0.5 um. Using the Weisz theory., the authors could predict the catalytic efficiency, assuming that the average length of the diffusion path was half the dimension of the crystals along the b-axis. Following the present synthesis route, we have shown that it was possible to prepare TS-1 crystals with well developed (ac) planes and a dimension along the b-axis of 0.3-0.4 ,urn (sample 1), thus leading to an average length of the diffusion path of 0.15-0.2 um. Therefore, these TS-1 samples are expected to have a catalytic efficiency similar to that of conventional TS-1 crystals of 0.3-0.4 um diameter. Results of the hydroxylation of phenol over sample 1 are reported in Table 3 and compared with those obtained over the standard TS-1. Results show that sample 1 is active in this reaction and that the p/o ratio at the end of the reaction is higher than that obtained over the standard TS-1. This can be attributed to the lower external surface of sample 1 as compared to the standard TS-1 (about half that of TS-1, as estimated from SEM pictures). Indeed, we have reported that catechol, the ortho isomer, was preferentially formed on the surface sites of the crystals whereas hydroquinone, the para isomer, was essentially formed inside the channels [10]. Table 3 Hydroxylation of phenol over sample 1 and a conventional TS-1 sample. Sample
t (min)
Cph (%)
SH202 (%)
CAT (%)
HYD (%)
HYD/CAT
1
60 120
15 19
65 90
4 5
10 13
2.5 2.6
TS-1
60
20
95
6.5
12.5
1.9
Cph is the phenol conversion and SH20 2 the selectivity in dihydroxybenzenes. CAT: catechol, HYD: hydroquinone
268 4. CONCLUSION We have shown that it is possible to synthesize highly crystalline TS-1 from gels containing hexanediamine and TPABr as