The first edition was published as Polysaccharides: Structural Diversity and Functional Versatility, edited by Severian ...
59 downloads
2177 Views
59MB Size
Report
This content was uploaded by our users and we assume good faith they have the permission to share this book. If you own the copyright to this book and it is wrongfully on our website, we offer a simple DMCA procedure to remove your content from our site. Start by pressing the button below!
Report copyright / DMCA form
The first edition was published as Polysaccharides: Structural Diversity and Functional Versatility, edited by Severian Dumitriu (Marcel Dekker, Inc., 1998). Although great care has been taken to provide accurate and current information, neither the author(s) nor the publisher, nor anyone else associated with this publication, shall be liable for any loss, damage, or liability directly or indirectly caused or alleged to be caused by this book. The material contained herein is not intended to provide specific advice or recommendations for any specific situation. Trademark notice: Product or corporate names may be trademarks or registered trademarks and are used only for identification and explanation without intent to infringe. Library of Congress Cataloging-in-Publication Data A catalog record for this book is available from the Library of Congress. ISBN: 0-8247-5480-8 This book is printed on acid-free paper. Headquarters Marcel Dekker 270 Madison Avenue, New York, NY 10016, U.S.A. tel: 212-696-9000; fax: 212-685-4540 Distribution and Customer Service Marcel Dekker Cimarron Road, Monticello, New York 12701, U.S.A. tel: 800-228-1160; fax: 845-796-1772 World Wide Web http://www.dekker.com The publisher offers discounts on this book when ordered in bulk quantities. For more information, write to Special Sales/Professional Marketing at the headquarters address above. Copyright n 2005 by Marcel Dekker. All Rights Reserved. Neither this book nor any part may be reproduced or transmitted in any form or by any means, electronic or mechanical, including photocopying, microfilming, and recording, or by any information storage and retrieval system, without permission in writing from the publisher. Current printing (last digit): 10 9 8 7 6 5 4 3 2 1 PRINTED IN THE UNITED STATES OF AMERICA
Foreword
Polysaccharides as natural polymers are by far the most abundant renewable resource on the earth with an annual formation rate surpassing the world production rate of synthetic polymers by some orders of magnitude. In contrast to petroleum-based synthetic polymers, plant polysaccharides are sustainable materials synthesized by the sun’s energy and fully biodegradable in the original state. Thus, with decreasing supply of oil resources polysaccharides, including cellulose, starch, chitin, and hemicelluloses, are expected to play an increasingly important role in industrial use. Polysaccharides are designed by nature to carry out various specific functions. Examples comprise structural polymers such as cellulose and chitin, storage polysaccharides such as starch and glycogen, and gel forming mono- and copolymers such as mucopolysaccharides (glycosaminoglycans), agar, and pectins. Generally, polysaccharides are highly functional polymers with magnificent structural diversity and functional versatility. Their structural and functional properties are often superior to synthetic materials as demonstrated, for instance, by the cellulose based cell wall architecture of plants or the function of hyaluronic acid in the human body. It has been a true challenge to present state-of-the-art polysaccharide research from different aspects regarding the macromolecular variety, function and structure in just one volume. In this book well-known and recognized authors describe the current state of research in their specific fields of expertise in which many of them have been active for decades. With regard to cellulose and starch as the most abundant polysaccharides, structure, chemical modification, physical chemistry, and industrial aspects are being discussed. It is further demonstrated that cellulosic biomass conversion technology permits large scale sustainable production of basic chemicals and derived products. The focus of other chapters are bacterial polysaccharides, hemicelluloses, gums, chitin, chitosan, hyaluronan, alginates, proteoglycans, glycolipides, and heparan sulfate-like polysaccharides. Some chapters deal with medical and pharmaceutical aspects including medical foods, anticoagulant properties and the role of polysaccharides in tissue engineering. Furthermore, methodical aspects, including characterization by X-ray scattering, spectroscopic methods, light scattering, and rheology are discussed. In summary, the comprehensive, improved, and expanded second edition of ‘‘Polysaccharides’’ reflects the current state of knowledge of nearly the entire spectrum of polysaccharides with emphasis on structures, methods of structural analysis, functions and properties, novel routes of modification, and novel application fields. With each chapter, the reader will find references for a deeper insight into a specific field. Thus, this book is a very useful tool for scientists of both academia and industry interested in the fundamental principles of polysaccharide functions and modifications on one hand and novel applications on the other. Having been involved in similar work mainly with industry-related issues of cellulose research for many years, I would like to stress that the presented state of knowledge, as sophisticated as it might seem to be, should not be understood as the final stage, but as an invitation to add new knowledge to this field and to explore additional applications of polysaccharides. I would be delighted, if this monograph challenged and encouraged scientists to deal with polysaccharides as fascinating polymers with a bright future. Hans-Peter-Fink Fraunhofer-Institute for Applied Polymer Research Potsdam-Golm, Germany iii
Preface
Polysaccharides are the macromolecules that belong to the means components of life. Together with nucleic acids and proteins, the polysaccharides determine the functionality and specificity of the species. Polysaccharides have received little such promotion even though they are widely distributed throughout nature and have highly organized structure. There are important molecules involved throughout the body in signal transduction and cell adhesion. Polysaccharides can be broadly classified into three groups based on their functions, which are closely related to their occurrence in nature: structural, storage, and gel forming. The first compounds used at the industrial level were the polysaccharides. This work provides the most complete summary now available of the present knowledge of polysaccharide chemistry. This book discusses eleven fundamental aspects of polysaccharides: 1. Progress in structural characterization. The structural analysis may offer the most fundamental knowledge to understand the functions of polysaccharides, but the diversity and irregularity of polysaccharide chains make the structural analysis a formidable task. The conformational analysis involves two aspects: (a) the characterization of a single chain conformation and (b) the analysis of the chain assembly of polysaccharides. A remarkable progress has been achieved in recent years with high-resolution, solution- and solid-state-1H- and 13C-NMR including cross-polarization-magic-angle-spinning and two-dimensional techniques. Specific electron microscopy techniques can visualize single polysaccharide molecules and can yield reliable information on their contour length distribution, persistence length and conformational aspects. Some recent progress reports on computational methods for simulations and calculations associated with structure elucidation of polysaccharides have demonstrated that these methods can contribute to a ‘‘decision’’ on the actual conformational properties of oligosaccharides and linear polysaccharides. 2. Conformation and dynamic aspects of polysaccharide gels. The most important aspect of characterization of polysaccharide gels seems to clarify their backbone dynamics together with conformations as viewed from their highly heterogeneous nature. Backbone dynamics of polysaccharide gel network can be characterized by means of simple comparative high-resolution 13C NMR measurements by cross-polarization-magic angle spinning (CP-MAS) and dipolar decoupled-magic angle spinning (DD-MAS) techniques. 3. Rheological behavior of polysaccharides in aqueous systems. Rheology provides precious tools to explore and understand the properties of polysaccharides in aqueous systems. The rheological behavior of polysaccharides systems manifests the underlying structure of the systems. In the simplest case, that of polysaccharides solution, viscosity is directly related to fundamental molecular properties (molecular conformations, molecular weight and molecular weight distribution, intramolecular and intermolecular interactions). In the case of more structured polymer systems, gels, for example, their viscoelastic properties are related to supramolecular organization. The main types of polysaccharide systems that are encountered in the applications can be distributed schematically in three classes: solutions, gels, and polysaccharide/ polysaccharide (or polysaccharide/protein) mixtures in aqueous media. 4. Biosynthesis, structure, and physical properties of bacterial polysaccharides (exopolysaccharides). This part presents the mechanisms of biosynthesis of bacterial polysaccharides and provides some information on the engineering of polysaccharides that will allow in the near future the production of a polysaccharide with a choice chemical structure having a set of predictable physical properties. This part covers also pertinent areas such as: bacterial and fungal polysaccharides, cell-wall polysaccharides, production of microbial polysaccharides, industrial gums, and microbial exopolysaccharides of practical importance. v
vi
Preface
The bacterial polysaccharides are described as: production and synthesis, composition and structure, physical properties, degradation by polysaccharases and polysaccharide lyases, polysaccharides common to prokaryotes and eukaryotes, biological properties and applications and commercial products. One chapter is dedicated to the presentation of the order-disorder conformational transition of xanthan gum. 5. Hemicelluloses may function both as framework and matrix substances or reserve substances in seeds, where they form independent wall layers which are mobilized when the seed germinates. In both hardwood and softwood, hemicelluloses fraction in lignified cell walls represents the matrix substance. This important part of the polysaccharides chemistry is presented in three chapters: Hemicelluloses: Structure and properties; Chemical modification of hemicelluloses and gums; Role of acetyl substitution in hardwood xylan. 6. In this edition a particular emphasis is placed on the presentation of the ionic polysaccharides (polyanion and polycation) in the following chapters: Alginate—A polysaccharide of industrial interest and diverse biological functions; Characterization and properties of hyaluronic acid (hyaluronan); Structure – property relationship in chitosans; Chitosan as a delivery system for transmucosal administration of drugs; Pharmaceutical applications of chitosan; Macromolecular complexes of chitosan. 7. Cellulose and starch are the two polysaccharides which constitute the majority of the polysaccharide production. They are presented in four chapters: Chemical functionalization of cellulose; The physical chemistry of starch; Starch: commercial sources and derived products; New development in cellulose technology. 8. The polysaccharides of a major importance in medicine and biology are extensively discussed in nine chapters: Polysialic acid: structure and properties; Brain proteoglycans; Crystal structures of glycolipids; Synthetic and natural polysaccharides with anticoagulant properties; Structural elucidation of heparan sulfate-like polysaccharides using miniaturized LC/MS; Enzymatic synthesis of heparan sulfate; Synthetic and natural polysaccharides having biological activities; Polysaccharide-based hydrogels in tissue engineering and Medical foods and fructooligosaccharides. Polysialic acids form a structurally unique group of linear carbohydrate chains with a degree of polymerization up to 200 sialyl residue. Polysialic acids chains are covalently attached to membrane glycoconjugates on cells that range in evolutionary diversity from bacteria to human brains. Proteoglycans, a group of glycoproteins that are invested with covalently bound glycosaminoglycan chains, are one of the important classes of molecules in brain development and maturation. The glycosaminoglycan chains that define proteoglycans are of four major classes: heparan sulfate; chondroitin sulfate, dermatan sulfate and keratan sulfate. The glycolipids play roles as the structural holder of membrane proteins suspended in bilayer or bicontinuous cubic phases and as the key code of the intercellular communication or immune system. Anticoagulant polysaccharides as heparin, heparan sulfate and nonheparin glycosaminoglycans (dermatan sulfate, chondroitin sulfates, acharan sulfate, carrageenas, sulfated fucans, sulfated galactan and nonheparin glycosaminoglycans from microbial sources) have been of interest to the medical profession. 9. Renewable resources. Cellulosic biomass includes agricultural (e.g., corn stover and sugarcane bagase) and forestry (e.g., sawdust, thin-nings, and mill wastes) residues, portions of municipal solid waste (e.g., waste paper) and herbaceous (e.g., switch-grass) and woody (e.g., poplar trees) corps. They are appropriate materials used as renewable resources for the production of building blocks for various industrial chemicals and engineering plastics polysaccharides. The chapters ‘‘Bioethanol production from lignocellulosic material’’, and Cellulosic biomass-derived products, describe and evaluate the process for ethanol fuel production. The raw material, hydrolysis, and fermentation are described in detail as well as the different possibilities to perform these process steps in various process designs. The chapter ‘‘Hydrolysis of cellulose and hemicellulose’’ presents a comprehensive overview of the technology and economic status for cellulose and hemicellulose hydrolysis describes the important structural features of cellulosic materials, applications, process steps, and stoichiometry for hydrolysis reactions. The chapter then examines biomass structural characteristics that influence cellulose hydrolysis by enzymes, types of cellulose hydrolysis processes, experimental results for enzymatic conversion of cellulose, and summarizes some of the factors influencing hydrolysis kinetics. 10. New applications of polysaccharides. This section provides a selection of some new developmental products and some recent applications, which might become of commercial interest in the near future. The polysaccharides are utilized as gallants, thickeners, film formers, fillers, and delivery systems in pharmaceutical and cosmetic applications. Immobilization. The use of ionic polysaccharides for the immobilization (enzymes, cells and other biocatalysts for biotechnological production) Ligand systems. Chitin, chitosan and other functional polysaccharides have also been widely used for the preparation of metal chelators. Industrial application ranges from waste water treatment, ion exchange resins, and precious metal recovery. Separatory systems. Cellulose and chitosan derivatives are dominating the membrane market due to their favorable stability and their selectivity in gas- and liquid-phase separations. Biosurfactants. Numerous microorganisms (candida lipolytica, Acetinobacter calcoaceticus) produce extracellular glycoconjugates with pronounced capabilities to modify interfacial and surface conditions. Cellulose derivative composites for electro-optical applications. These studies present an optical cell formed by a transparent solid matrix of mixed esters of cellulose with micrometer-sized pores filled with a nemantic liquid crystal.
Preface
vii
11. Incorporation of the polysaccharides in the synthetic matrix offers on one hand the possibility to obtain a broader application range of the usual polymers and, on the other hand, ways to optimize and control some properties and produce new materials with unexpected performance at low cost. The treatise is truly international with authors now residing in Austria, Brazil, Canada, Denmark, Egypt, Finland, France, Germany, Greece, Japan, The Netherlands, Norway, Portugal, Romania, Sweden, United Kingdom, and the United States. The editor is grateful to all the collaborators for their precious contributions. Severian Dumitriu
Contents
Foreword Hans-Peter-Fink Preface Contributors 1. Progress in Structural Characterization of Functional Polysaccharides Kanji Kajiwara and Takeaki Miyamoto
iii v xiii 1
2. Conformations, Structures, and Morphologies of Celluloses Serge Pe´rez and Karim Mazeau
41
3. Hydrogen Bonds in Cellulose and Cellulose Derivatives Tetsuo Kondo
69
4. X-ray Diffraction Study of Polysaccharides Toshifumi Yui and Kozo Ogawa
99
5. Recent Developments in Spectroscopic and Chemical Characterization of Cellulose Rajai H. Atalla and Akira Isogai
123
6. Two-Dimensional Fourier Transform Infrared Spectroscopy Applied to Cellulose and Paper Lennart Salme´n, Margaretha A˚kerholm, and Barbara Hinterstoisser
159
7. Light Scattering from Polysaccharides Walther Burchard
189
8. Advances in Characterization of Polysaccharides in Aqueous Solution and Gel State M. Rinaudo
237
9. Conformational and Dynamics Aspects of Polysaccharide Gels by High-Resolution Solid-State NMR Hazime Saitoˆ
253
10.
Correlating Structural and Functional Properties of Lignocellulosics and Paper by Fluorescence Spectroscopy and Chemometrics Emmanouil S. Avgerinos, Evaggeli Billa, and Emmanuel G. Koukios
267
ix
x
Contents
11.
Computer Modeling of Polysaccharide–Polysaccharide Interactions Francßois R. Taravel, Karim Mazeau, and Igor Tvarosˇka
281
12.
Interactions Between Polysaccharides and Polypeptides Delphine Magnin and Severian Dumitriu
305
13.
Rheological Behavior of Polysaccharides Aqueous Systems Jacques Lefebvre and Jean-Louis Doublier
357
14.
Stability and Degradation of Polysaccharides Valdir Soldi
395
15.
Biosynthesis, Structure, and Physical Properties of Some Bacterial Polysaccharides Roberto Geremia and Marguerite Rinaudo
411
16.
Microbial Exopolysaccharides I. W. Sutherland
431
17.
Order–Disorder Conformational Transition of Xanthan Gum Christer Viebke
459
18.
Hemicelluloses: Structure and Properties Iuliana Spiridon and Valentin I. Popa
475
19.
Chemical Modification of Hemicelluloses and Gums Margaretha So¨derqvist Lindblad and Ann-Christine Albertsson
491
20.
Role of Acetyl Substitution in Hardwood Xylan Maria Gro¨ndahl and Paul Gatenholm
509
21.
Alginate—A Polysaccharide of Industrial Interest and Diverse Biological Functions Wael Sabra and Wolf-Dieter Deckwer
515
22.
Characterization and Properties of Hyaluronic Acid (Hyaluronan) Michel Milas and Marguerite Rinaudo
535
23.
Chemical Functionalization of Cellulose Thomas Heinze
551
24.
The Physical Chemistry of Starch R. Parker and S. G. Ring
591
25.
Starch: Commercial Sources and Derived Products Charles J. Knill and John F. Kennedy
605
26.
Structure–Property Relationship in Chitosans Kjell M. Va˚rum and Olav Smidsrød
625
27.
Chitosan as a Delivery System for the Transmucosal Administration of Drugs Lisbeth Illum and Stanley (Bob) S. Davis
643
28.
Pharmaceutical Applications of Chitosan and Derivatives M. Thanou and H. E. Junginger
661
29.
Macromolecular Complexes of Chitosan Naoji Kubota and Kei Shimoda
679
30.
Polysialic Acid: Structure and Properties Tadeusz Janas and Teresa Janas
707
Contents
xi
31.
Brain Proteoglycans Russell T. Matthews and Susan Hockfield
729
32.
Crystal Structures of Glycolipids Yutaka Abe and Kazuaki Harata
743
33.
Synthetic and Natural Polysaccharides with Anticoagulant Properties Fuming Zhang, Patrick G. Yoder, and Robert J. Linhardt
773
34.
Structural Elucidation of Heparan Sulfate-Like Polysaccharides Using Miniaturized LC/MS Balagurunathan Kuberan, Miroslaw Lech, and Robert D. Rosenberg
795
35.
Enzymatic Synthesis of Heparan Sulfate Balagurunathan Kuberan, David L. Beeler, and Robert D. Rosenberg
811
36.
Polysaccharide-Based Hydrogels in Tissue Engineering Hyunjoon Kong and David J. Mooney
817
37.
Synthetic and Natural Polysaccharides Having Specific Biological Activities Takashi Yoshida
839
38.
Medical Foods and Fructooligosaccharides Bryan W. Wolf, JoMay Chow, and Keith A. Garleb
853
39.
Immobilization of Cells in Polysaccharide Gels Yunyu Yi, Ronald J. Neufeld, and Denis Poncelet
867
40.
Hydrothermal Degradation and Fractionation of Saccharides and Polysaccharides Ortwin Bobleter
893
41.
Cellulosic Biomass-Derived Products Charles J. Knill and John F. Kennedy
937
42.
Bioethanol Production from Lignocellulosic Material Lisbeth Olsson, Henning Jørgensen, Kristian B. R. Krogh, and Christophe Roca
957
43.
Hydrolysis of Cellulose and Hemicellulose Charles E. Wyman, Stephen R. Decker, Michael E. Himmel, John W. Brady, Catherine E. Skopec, and Liisa Viikari
995
44.
New Development in Cellulose Technology Bruno Lo¨nnberg
1035
45.
Polysaccharide Surfactants: Structure, Synthesis, and Surface-Active Properties Roger E. Marchant, Eric H. Anderson, and Junmin Zhu
1055
46.
Structures and Functionalities of Membranes from Polysaccharide Derivatives Tadashi Uragami
1087
47.
Electro-optical Properties of Cellulose Derivative Composites J. L. Figueirinhas, P. L. Almeida, and M. H. Godinho
1123
48.
Blends and Composites Based on Cellulose Materials Georgeta Cazacu and Valentin I. Popa
1141
49.
Preparation and Properties of Cellulosic Bicomponent Fibers Richard D. Gilbert and John F. Kadla
1179
Index
1189
Contributors
Yutaka Abe
Process Development Research Center, Lion Corporation, Tokyo, Japan
Margaretha A˚kerholm STFI (Swedish Pulp and Paper Research Institute), Stockholm, Sweden Ann-Christine Albertsson
Royal Institute of Technology, Stockholm, Sweden
P. L. Almeida EST/IPS, Setu´bal, Portugal and FCT/UNL, Caparica, Portugal Case Western Reserve University, Cleveland, Ohio, U.S.A.
Eric H. Anderson Rajai H. Atalla
USDA Forest Service and University of Wisconsin, Madison, Wisconsin, U.S.A.
Emmanouil S. Avgerinos
National Technical University of Athens, Athens, Greece
David L. Beeler Massachusetts Institute of Technology, Cambridge, Massachusetts, U.S.A. and Beth Israel Deaconess Medical Center, Harvard Medical School, Boston, Massachusetts, U.S.A. Evaggeli Billa
National Technical University of Athens, Athens, Greece
Ortwin Bobleter University of Innsbruck, Innsbruck, Austria John W. Brady
Cornell University, Ithaca, New York, U.S.A.
Walther Burchard
Institute of Macromolecular Chemistry, University of Freiburg, Germany
Georgeta Cazacu ‘‘Petru Poni’’ Institute of Macromolecular Chemistry, Iasi, Romania JoMay Chow
Abbott Laboratories, Columbus, Ohio, U.S.A.
Stanley (Bob) S. Davis University of Nottingham, Nottingham, United Kingdom xiii
xiv
Contributors
Stephen R. Decker National Renewable Energy Laboratory, Golden, Colorado, U.S.A. Biochemical Engineering, GBF–National Research Center for Biotechnology, Braunschweig,
Wolf-Dieter Deckwer Germany
INRA-Laboratoire de Physico-Chimie des Macromole´cules, Nantes, France
Jean-Louis Doublier Severian Dumitriu
Sherbrooke University, Sherbrooke, Quebec, Canada
J. L. Figueirinhas
CFMC/UL, Lisbon, Portugal
Keith A. Garleb Abbott Laboratories, Columbus, Ohio, U.S.A. Paul Gatenholm Biopolymer Technology, Department of Materials and Surface Chemistry, Chalmers University of Technology, Go¨teborg, Sweden Roberto Geremia Laboratoire d’Adaptation et de Pathoge´nie des Microorganismes, Joseph Fourier University, Grenoble, France Richard D. Gilbert
North Carolina State University, Raleigh, North Carolina, U.S.A.
FCT/UNL, Caparica, Portugal
M. H. Godinho
Maria Gro¨ndahl Biopolymer Technology, Department of Materials and Surface Chemistry, Chalmers University of Technology, Go¨teborg, Sweden Kazuaki Harata Biological Information Research Center, National Institute of Advanced Industrial Science and Technology, Ibaraki, Japan Thomas Heinze Center of Excellence for Polysaccharide Research at the Friedrich Schiller University of Jena, Jena, Germany Michael E. Himmel
National Renewable Energy Laboratory, Golden, Colorado, U.S.A.
Barbara Hinterstoisser Susan Hockfield
Yale University School of Medicine, New Haven, Connecticut, U.S.A.
IDentity, Nottingham, United Kingdom
Lisbeth Illum Akira Isogai
BOKU-University of Natural Resources and Applied Life Sciences, Vienna, Austria
Graduate School of Agricultural and Life Science, University of Tokyo, Tokyo, Japan
Tadeusz Janas Teresa Janas
University of Colorado, Boulder, Colorado, U.S.A. University of Colorado, Boulder, Colorado, U.S.A. and University of Zielona, Go´ra, Poland
Henning Jørgensen
Center for Microbial Biotechnology BioCentrum-DTU, kgs. Lyngby, Denmark
H. E. Junginger Leiden University, Leiden, The Netherlands John F. Kadla North Carolina State University, Raleigh, North Carolina, U.S.A. Kanji Kajiwara
Otsuma Women’s University, Chiyoda-ku, Tokyo, Japan
Contributors
xv
John F. Kennedy Kingdom
University of Birmingham Research Park and Chembiotech Laboratories, Birmingham, United
Charles J. Knill Kingdom
University of Birmingham Research Park and Chembiotech Laboratories, Birmingham, United
Kyushu University, Fukuoka, Japan
Tetsuo Kondo
University of Michigan, Ann Arbor, Michigan, U.S.A.
Hyunjoon Kong
Emmanuel G. Koukios
National Technical University of Athens, Athens, Greece
Kristian B. R. Krogh Center for Microbial Biotechnology BioCentrum-DTU, kgs. Lyngby, Denmark Balagurunathan Kuberan Massachusetts Institute of Technology, Cambridge, Massachusetts, U.S.A. and Beth Israel Deaconess Medical Center, Harvard Medical School, Boston, Massachusetts, U.S.A. Oita University, Oita, Japan
Naoji Kubota
Miroslaw Lech Massachusetts Institute of Technology, Cambridge, Massachusetts, U.S.A. and Beth Israel Deaconess Medical Center, Harvard Medical School, Boston, Massachusetts, U.S.A. Jacques Lefebvre INRA-Laboratoire de Physico-Chimie des Macromole´cules, Nantes, France Margaretha So¨derqvist Lindblad
Royal Institute of Technology, Stockholm, Sweden
Robert J. Linhardt University of Iowa, Iowa City, Iowa, U.S.A. A˚bo Akademi University, Turku/A˚bo, Finland
Bruno Lo¨nnberg
Sherbrooke University, Sherbrooke, Quebec, Canada
Delphine Magnin Roger E. Marchant
Case Western Reserve University, Cleveland, Ohio, U.S.A.
Russell T. Matthews Yale University School of Medicine, New Haven, Connecticut, U.S.A. Centre de Recherches sur les Macromole´cules Ve´ge´tales, Grenoble, France
Karim Mazeau
Michel Milas Centre de Recherches sur les Macromole´cules Ve´ge´tales (CERMAV), CNRS, and Joseph Fourier University, Grenoble, France Takeaki Miyamoto David J. Mooney Ronald J. Neufeld Kozo Ogawa
National Matsue Polytechnic College, Matsue, Japan University of Michigan, Ann Arbor, Michigan, U.S.A. Queen’s University, Kingston, Ontario, Canada
Osaka Prefecture University, Sakai, Osaka, Japan
Lisbeth Olsson Center for Microbial Biotechnology BioCentrum-DTU, kgs. Lyngby, Denmark R. Parker Serge Pe´rez
Institute of Food Research, Norwich Research Park, Norwich, United Kingdom Centre de Recherches sur les Macromole´cules Ve´ge´tales, Grenoble, France
xvi
Contributors
ENITIAA, Nantes, France
Denis Poncelet
Technical University of Jassy, Jassy, Romania
Valentin I. Popa
Marguerite Rinaudo Centre de Recherches sur les Macromole´cules Ve´ge´tales (CERMAV), CNRS, and Joseph Fourier University, Grenoble, France Institute of Food Research, Norwich Research Park, Norwich, United Kingdom
S. G. Ring
Center for Microbial Biotechnology BioCentrum-DTU, kgs. Lyngby, Denmark
Christophe Roca
Robert D. Rosenberg Massachusetts Institute of Technology, Cambridge, Massachusetts, U.S.A. and Beth Israel Deaconess Medical Center, Harvard Medical School, Boston, Massachusetts, U.S.A. Microbiology Department, Faculty of Science, Alexandria University, Alexandria, Egypt
Wael Sabra
Hazime Saitoˆ Himeji Institute of Technology, Kamigori, Hyogo, Japan and Center for Quantum Life Sciences, Hiroshima University, Higashi-Hiroshima, Japan STFI (Swedish Pulp and Paper Research Institute), Stockholm, Sweden
Lennart Salme´n
Kei Shimoda Oita University, Oita, Japan Catherine E. Skopec Cornell University, Ithaca, New York, U.S.A. Norwegian University of Science and Technology (NTNU), Trondheim, Norway
Olav Smidsrød
Valdir Soldi Federal University of Santa Catarina, Floriano´polis, SC, Brazil Iuliana Spiridon ‘‘Petru Poni’’ Institute of Macromolecular Chemistry, Jassy, Romania University of Edinburgh, Edinburgh, United Kingdom
I. W. Sutherland
Franc¸ois R. Taravel Centre de Recherches sur les Macromole´cules Ve´ge´tales (CERMAV), CNRS, and Joseph Fourier University, Grenoble, France Cardiff University, Cardiff, United Kingdom
M. Thanou
Institute of Chemistry, Slovak Academy of Sciences, Bratislava, Slovakia
Igor Tvarosˇ ka
Kansai University, Osaka, Japan
Tadashi Uragami Kjell M. Va˚rum
Norwegian University of Science and Technology (NTNU), Trondheim, Norway
Christer Viebke Kingdom
The North East Wales Institute, Water Soluble Polymers Group Plas Coch, Wrexham, United
Liisa Viikari
VTT Technical Research Centre of Finland, Finland
Bryan W. Wolf
Abbott Laboratories, Columbus, Ohio, U.S.A.
Charles E. Wyman Yunyu Yi
Dartmouth College, Hanover, New Hampshire, U.S.A.
Queen’s University, Kingston, Ontario, Canada
Contributors
xvii
Patrick G. Yoder University of Iowa, Iowa City, Iowa, U.S.A. Takashi Yoshida
Kitami Institute of Technology, Kitami, Japan
Toshifumi Yui
Miyazaki University, Miyazaki, Japan
Fuming Zhang
University of Iowa, Iowa City, Iowa, U.S.A.
Junmin Zhu
Case Western Reserve University, Cleveland, Ohio, U.S.A.
1 Progress in Structural Characterization of Functional Polysaccharides Kanji Kajiwara Otsuma Women’s University, Chiyoda-ku, Tokyo, Japan
Takeaki Miyamoto National Matsue Polytechnic College, Matsue, Japan
I. INTRODUCTION Oligosaccharides and polysaccharides are biopolymers commonly found in living organisms, and are known to reveal the physiological functions by forming a specific conformation. However, our understanding of polysaccharide chains is still in its premature state with respect to their structure in solid and in solution. Structural analysis may offer the most fundamental knowledge to understand the functions of polysaccharides, but the diversity and irregularity of polysaccharide chains make it a formidable task. Polysaccharide chains are partly organized but are considered to be mostly amorphous. No single crystal was made from polysaccharides up to now. Thus the crystallographic analysis of polysaccharide chains has been performed by either using the small oligosaccharide single crystals or the x-ray fiber pattern diffraction from drawn polysaccharide gels. Although a monosaccharide unit is common to many polysaccharides, its linkage mode varies and characteristic functions/properties will appear accordingly. A good example is demonstrated by simple poly-D-glucans—water-soluble, digestible amylose and non-water-soluble, nondigestible cellulose. Both amylose and cellulose are homopolymers composed of glucosidic residues, but they differ in the mode of linkage. Amylose is a (1!4)-a-Dlinked polyglucan, whereas cellulose is a (1!4)-a-Dlinked polyglucan. The (1!4)-a linkage (amylose) and the (1!4)-a linkage (cellulose) of D-glucosidic residues yield a wobbled helix and a stretched zigzag chain, respectively, by joining the D-glucosidic residues in a simple manner so as to place the chain on a plane [1]
(Fig. 1). In later sections, it will be shown that these basic conformations of amylose and cellulose are supposed to be retained to some extent in aqueous solutions. The difference in the structure is reflected by the respective physiological functions of edible amylose and nonedible cellulose. There are some evidences that the higher-order structure of polysaccharide chains is related to their physiological function as exemplified by the triple-stranded helix of scleroglucan, which is known to possess an antitumor activity. Many polysaccharide chains are able to assume an ordered or quasi-ordered structure such as a doublestranded helix, but the ordered structure is interrupted by the irregularity of the primary structure in the polysaccharide chains. Many polysaccharide chains form gel in solutions by assuming an ordered or quasi- ordered chain structure, which constitutes a cross-linking domain. The conformational analysis of polysaccharide chains involves two aspects: (1) the characterization of a single chain conformation and (2) the analysis of the chain assembly (suprastructure) of polysaccharides. A single chain conformation of polysaccharides is primarily determined by the chemical structure specified by the types of sugar residues, sugar linkages, and side groups. A single chain conformation accounts, to some extent, for the formation of suprastructures such as the complexing capability of amylose and the fringed micelle formation of cellulose. Unlike cellulose and amylose, most polysaccharides have no regular homopolymeric structure, where the regularity is interrupted by the random intrusion of different types of linkage and/or sugar units. The introduction of 1
2
Kajiwara and Miyamoto
Figure 1 Wobbled helical conformation (a) and stretched zigzag conformation (b), representing the basic conformations of amylose and cellulose, respectively.
such an irregularity hampers crystallization and promotes the formation of a suprastructure that is characteristic of the polysaccharide species. The interchain interaction of polysaccharides seems to be specific as exemplified by the suprastructure depending on the chemical structure and counterions (in the case of polysaccharides possessing carboxyl or sulfate groups). The formation of the suprastructure often results to gelation. The complexity in characterizing polysaccharide chain conformation is due to the fact that the interchain interaction of polysaccharides is so specific that polysaccharide chains are seldom dispersed in solvent as a single chain. Thus a first task to understand the structure–function relationship of polysaccharides is to evaluate the intrinsic chain (single chain) characteristics free from interchain interaction. Once the intrinsic chain conformation is specified, the interchain interaction can be analyzed in terms of the mode of suprastructure composed of several polysaccharide chains. This review is intended to demonstrate the recent strategy in the structural and conformational characterization of oligosaccharides and polysaccharides. Although various techniques are applied for the structural and conformational analysis of oligosaccharides and polysaccharides, the general inability to crystallize excludes the
potential application of the crystallographic approach, which has been a main method of the structural analysis in protein science. Here we will describe two methods that are currently applied to the structural and conformational analysis of oligosaccharides and polysaccharides: smallangle x-ray scattering (SAXS) [2] and nuclear magnetic resonance (NMR) [3]. Molecular modeling by computer is considered to supplement the analysis by small-angle x-ray scattering and NMR. Although an initial intention of molecular modeling is to predict physical properties of carbohydrates a priori [4], the ab initio calculation is limited to a small monosaccharide and the semiempirical quantum method can be applied for the structural characterization of molecules up to the size of disaccharides. Molecular mechanics or molecular dynamics is an alternative method applied to the computer modeling of larger carbohydrate molecules, where the motion of constituent atoms is assumed to be described in terms of classical mechanics. In the final chapter, the structural and conformational aspect is discussed from the chemical point of view. Here the controlled chemical modification of cellulose is treated and the physicochemical characteristics are discussed by taking into account the structural change due to chemical modification of cellulose.
Progress in Structural Characterization of Functional Polysaccharides
II. STRATEGY AND METHODS OF ANALYSIS Because many monosaccharides have a single, well-established conformation, the conformational analysis of oligosaccharides and polysaccharides starts from understanding the energetic relationship when the monosaccharide residues are linked in a specific way. The entire geometry of oligosaccharides and polysaccharide chains can be described in terms of a set of the pairs of dihedral angles of rotation about the monosaccharide links. If the rotation is independent at each monosaccharide link, the chain should assume a random coil conformation. However, the conformation of saccharide chains is found in most cases to assume nonrandom conformations due to intra- and interchain interactions that suppress the conformational space available for the chains linked by independent rotation. Even the crystal structure is partly retained in solution as in the case of protein. Thus a single chain conformation may account, to some extent, for the mode of interactions and the formation of suprastructures. This section gives a brief introduction on the structure of monosaccharides and disaccharides as the basis of the structural and conformational analysis of oligosaccharides and polysaccharides. The fundamentals of SAXS and NMR together with the molecular modeling are also described.
A. Structure of Monosaccharide and Disaccharide A monosaccharide is given by the chemical formula CnH2nOn, where n = 3–10. Pentose (n = 5) and hexose (n = 6) are the most abundant in nature, and are composed of a pyranose or a furanose (Fig. 2) as a basic ring structure. A pyranose ring has two stable chair form (C) conformers C1 and 1C where four atoms of O, C2, C3, and C5 are on the same plane. Fig. 3 lists some of pyranose-type pentose and hexose, which appear in later sections, where the abbreviated description is given for each monosaccharide. A disaccharide is composed of two monosaccharides linked by any of the four modes of glycosidic linkages a,aV, a,hV, h,aV-, or h,hV-. Table 1 shows some disaccharides
Figure 2 Pyranose and furanose.
3
found in nature. The structural analysis of disaccharide implies the identification, the linking order, the link position, and the link mode of constituent monosaccharides. Chemical and optical methods are available to determine the structure of disaccharide, but the recent development in NMR has facilitated the assignment of specific protons or carbons as well as the conformational determination of the glucosidic linkage as shown in the next section. Fouriertransform infrared (FTIR) and laser Raman spectroscopy are also useful tools for the characterization of glycosidic bonds [5]. X-ray and neutron diffraction can be applied to determine the crystal structure and hydrogen bonding of monosaccharides and disaccharides that form a single crystal. A classic example will be found in the crystal structure analysis of h-maltose monohydrate [6] (Fig. 4), where the earlier structure determination using x-ray diffraction [7] was refined to give a more accurate description of the hydrogen bond structure. The x-ray diffraction analysis provides the most explicit information on structure in terms of the precise atomic coordinates. The Cambridge Structural Database lists the crystal structure of about 40 small oligosaccharides (cyclodextrins are omitted) including about 10 trisaccharides, 2 tetrasaccharides, and 1 hexasaccharide. Here a number of crystal structures of mono-, di-, and trisaccharides were determined from the acetate derivatives because the acetylated derivatives are found to crystallize more easily than original (untreated) oligosaccharides. (1!3)-h-D-glucopyranosyl residues consist of a main chain of a medically important class of polysaccharides including curdlan, lentinan, schizophyllan, scleroglucan, and grifolan, which possess branches at C6 (except for curdlan). Glcph 1!3 Glc disaccharides are systematically synthesized and the crystal structures are determined. A first attempt was made by Takeda et al. [8] on 3-O-h-D-glucopyranosyl-h-D-glucopyranose (h-D-laminarabiose) ethyl hepta-O-acetyl-h-D-laminarabioside [9], followed by Perez et al. [10] on octa-O-acetyl-h-D-laminarabiose), and by Lamba et al. [11] on (methyl hepta-Oacetyl-h-D-laminarabiose). Recently, 3-O-h-D-glucopyranosyl-h-D-glucopyranoside (methyl h-D-laminarabioside) [12] and methyl hepta-O-acetyl-h-D-laminarabioside [13] were prepared, and the crystal structures were determined by x-ray diffraction (Fig. 5). Table 2 summarizes two dihedral angles, / and w, with respect to the glycosidic bond for (1!3)-h-linked disaccharides, evaluated from the crystallographic data of laminarabiose and laminarabioside derivatives. Here the dihedral angles are taken as / = h[H(C1) ,C1 ,O1, C3V] and w = h[C1, O1, C3V, H(C3V)]. (See Sec. II.D for the definition of dihedral angles / and w.) The angle / is almost invariant around 45j regardless of the substituents, while the angle w is classified in two groups of around 45j and 8j. When the intramolecular hydrogen bond is formed between 04V and 05, the angle y assumes a negative value. The introduction of acetyl groups prevents the formation of intramolecular hydrogen bonds as seen from the stereoview of the molecular structures of methyl h-D-laminarabioside and methyl hepta-Oacetyl-h-D-laminarabioside in Fig. 5. The invariance of
4
Kajiwara and Miyamoto
Figure 3 Pyranose-type pentose and hexose.
the angle 4) is attributed to the exo-anomeric effect that restricts rotation around the bond between an anomeric carbon atom and a glycosidic oxygen atom [14].
B. Fundamentals of Small-Angle X-Ray Scattering [2] Small-angle x-ray scattering is characterized by its small scattering angle. A scattering process obeys a reciprocal law that relates the distance r in an ordinary (real) space with the scattering vector q in a Fourier (scattering) space by the phase factor defined by exp(q r); that is, the scattered intensity I( q) is given by the Fourier transformation of the electron density distribution in the object: ðl 4pr2 cðrÞ expðiq rÞdr ð1Þ IðqÞ ¼ V ¼ 0
Here the magnitude of the scattering vector is given by (4p / k) sin(h / 2) with k and h being the wavelength and the scattering angle, respectively. c(r) is a correlation function representing the average of the product of two electron density fluctuations at a distance r. The distance distribution function p(r) is defined as pðrÞ ¼ Vr2 cðrÞ
ð2Þ
which is characteristic of the shape of the scattering object. The phase difference between scattered rays becomes more prominent as the scattering angle increases. Thus the scattered intensity is maximum at zero scattering angle and proportional to the number of electrons in the object where the scattered rays are all in phase. The scattered intensity decreases with increasing scattering angle and diminishes at a scattering angle of the order of k / D, where k and D
Progress in Structural Characterization of Functional Polysaccharides
5
Table 1 Disaccharides in Nature Mode of linkage (1!4) Linkage
(1!6) Linkage
(1!3) Linkage
(1!2) Linkage
(1!1) Linkage
Common name
Structure
Origin
maltose cellobiose lactose xylobiose chitobiose cellobiouronic acid isomaltose gentiobiose melibiose planteobiose nigerose laminaribiose turanose hyalobiuronic acid chondrosine kojibiose sophorose sucrose a,a-trehalose
Glcpa 1 ! 4 Glc Glcph 1 ! 4 Glc Galph 1 ! 4 Glc Xylph 1 ! 4 Xyl GlcNh 1 ! 4 GlcN GlcUAph 1 ! 4 Glc Glcpa 1 ! 6 Glc Glcph 1 ! 6 Glc Galpa 1 ! 6 Glc Galpa 1 ! 6 Fruf Glcpa 1 ! 3 Glc Glcph 1 ! 3 Glc Glcpa 1 ! 3 Fruf GlcUAph 1 ! 3 GlcN GlcUAph 1 ! 3 GalN Glcpa 1 ! 2 Glc Glcph 1 ! 2 Glc Frufh 1 ! 2 aGlcp Glcpa 1 ! 1 aGlcp
starch cellulose mammal milk xylan chitin D. pneumoniae amylopectin, etc. gentianose raffinose planteose mutan laminaran meleziose (honey) hyaluronic acid chondroitin sulfate Aspergillus orryzae Sophora japonica beet sugar yeast
p and f denote pyranose and furanose, respectively.
denote the wavelength of an incident beam and the average diameter of scattering objects. When x-ray is used as an incident beam (k = 0.154 nm), the limiting scattering angle to be observed is approximately equal to 0.450 when D = 10 nm, or to 0.0450 when D = 100 nm. Because the phase factor exp(q r) can be replaced by its space average sin qr/qr for the statistically isotropic system according to Debye [15], Eq. (1) can be expanded in the series of q2 at very small angles by expanding the sine term to yield the particle scattering factor as ðl 1 4pr2 cðrÞ r2 dr=2 PðqÞuIðqÞ=Ið0Þ ¼ 1 q2 3 0 ð3Þ ð
(Rt) of a flat particle by describing approximately the scattering from the cross-section or the thickness in terms of the exponential form. The scattering factor of a rod-like particle (a cylinder) consists of two components of the height and the cross-section as p exp q2 R2c =2 ð6Þ Pcylinder ðqÞc 2Hq where 2H denotes the height of the cylinder. The scattering factor of a flat particle (a disk) is given by the product of two terms of the cross-sectional area and the thickness as Pdisk ðqÞc
l
4pr2 cðrÞdr þ Oðq4 Þ
0
where the second term on the right side represents the radius of gyration RG, that is ðl ðl pðrÞ r2 dr=2 pðrÞdr ð4Þ R2G ¼ 0
2p exp q2 R2t 2 Aq
ð7Þ
where A denotes the cross-sectional area. Equations (6) and (7) suggest that the cross-sectional radius of gyration Rc
0
in terms of the distance distribution function Eq. (2). The sine expansion of Eq. (3) is approximately closed in the exponential form, and the particle scattering factor is reduced to the Guinier approximation [2,16]: PðqÞcexpðq2 R2G =3Þ
ð5Þ
suggesting that the radius of gyration can be evaluated from the initial slope by plotting ln P( q) against q2 (the Guinier plot). A similar argument can be applied to evaluate the radius of gyration corresponding to the cross-section of a rod-like particle (Rc) or the thickness
Figure 4 Ref. 6.)
Stereoview of h-maltose monohydrate. (From
6
Kajiwara and Miyamoto
Figure 5
Stereoview of methyl h-D-laminarabioside (top) and methyl hepta-O-acetyl-a-D-laminarabioside (bottom).
Table 2 Dihedral Angles of the Glycosidic Linkage for Glcph 1!3 Glc Disaccharides Compound Methyl h-D-laminarabioside h-D-laminarabiose Methyl hepta-O-acetyl-h-D-laminarabioside Methyl hepta-O-acetyl-a-D-laminarabioside Octa-O-acetyl-h-D-laminarabioside Octa-O-acetyl-a-D-laminarabioside
/ = h[H(C1), C1, O1, C3V]
w = h[C1, O1, C3V, H(C3V)]
43 28 43 43 42 54
52 38 5 2 14 11
Progress in Structural Characterization of Functional Polysaccharides
and the thickness radius of gyration Rt are evaluated from the initial slope of the corresponding Guinier plots: ln qPcylinder ( q) plotted against q2 or ln q2Pdisk( q) plotted against q2. Although the polymeric chain has an approximate shape as represented by a sphere or an ellipsoid as a whole in solution, the density distribution is not homogeneous but decays exponentially from the center to the circumference. A simple Ornstein–Zemike type is generally applied to the density correlation function for a Gaussian chain: n cðrÞic expðr=nÞ r
ð8Þ
where c is a concentration of polymer chains and n is a correlation length specifying the range of effective density fluctuation. Introducing in Eq. (1) for a statistically isotropic system, Eq. (8) yields the scattering profile as IðqÞc
cn3 1 þ n2 q2
ð10Þ
Equation (10) yields the scattering profile as cn3
ð11Þ
ð1 þ n2 q2 Þ2
which exhibits a faster decay of the scattered intensity with q. The particle scattering from a single molecule is in principle calculated from the coordinates of the constituent atoms n X
g2i /2i ðqÞ þ 2
i¼1
n1 X n X t¼1 j¼iþ1
PðqÞ ¼ / ðqRÞ ¼
ð12Þ
where q denotes the magnitude of the scattering vector given by (4p / k) sin(h / 2) with k and h being the wavelength of the incident beam and scattering angle, respectively, and gi is an atomic scattering factor. dij is the distance between the ith and jth atoms, and the form factor for a single atom /i( q) is assumed to be given by the form factor for a sphere with a van deer Walls radius of the ith atom
ðRi qÞ3
ðRqÞ3
ð13Þ
where RI is the van deer Walls radius of the ith atom. If a molecule is rigid, the distance dij is fixed and Eq. (1) is
#2 ð14Þ
where R denotes the radius of a sphere. The observed scattering profile is compared with that calculated from an assumed triaxial model of a suitable dimension, which is supposed to be composed of associated oligosaccharides or polysaccharide chains. No interdomain (interparticular) interaction is considered in the above argument, and the scattering is considered to be due solely to an isolated domain (or an isolated particle). When the interdomain (interparticular) interaction becomes dominant, an interference peak will appear at the q range corresponding to the interaction distance in the scattering profile. If the interdomain (interparticular) interaction is isotropic and spherically symmetric, the scattering profile is decomposed into the product of two terms of the particle scattering factor P( q) and the interference SI( q) [16]: ð15Þ
where the interference term is written as SI ðqÞc
3½sinðRi qÞ ðRi qÞcosðRi qÞ
3ðsin Rq Rq cos RqÞ
IðqÞcPðqÞ SI ðqÞ
gi gj /i ðqÞ/j ðqÞ
sindij q dij q
/i ¼
" 2
cðrÞiexpðr=nÞ
IðqÞ ¼
equivalent to the particle scattering factor of such a molecule that freely moves in space. If a molecule (e.g., a flexible polymer molecule) has a large internal freedom, the distance dij fluctuates with time due to the internal motion of such a molecule. In this case, the particle scattering factor should be calculated as an average over a statistical ensemble generated by the Monte Carlo procedure [18,19] according to the conditional bond conformation probability [20]. When no molecular model is available, the scattering profile can be analyzed in terms of a triaxial body model of homogeneous density representing the shape of the object [21] or by assuming a suitable pair correlation function for the electron density distribution in the object [22]. The scattering factor is explicitly calculated for some homogeneous triaxial bodies including a sphere, an ellipsoid, a cylinder, and a prism. For example, the scattering factor for a sphere is given by Eq. (14) as
ð9Þ
The volume term V in Eq. (1) is replaced by cn3, which corresponds to the number of units in the correlated density fluctuation. Debye and Beuche [17] proposed a correlation function that specifies the density correlation for a randomly associated system:
IðqÞc
7
1 3=2
1 ð2pÞ
ðe=m1 ÞbðqÞ
ð16Þ
with e and m1 being a constant close to unity and the average volume allocated to each interacting domain, respectively. b( q) represents the interaction potential in the Fourier (scattering) space. When the interdomain interaction is given in terms of a hard-sphere repulsion, b( q) is represented by the scattering amplitude of a sphere, Eqs. (13) and (16) reduce to SI ðqÞc
1 1 þ 8ðm0 =m1 Þe/ð2qRÞ
ð17Þ
where m0 is the volume of the sphere and the hard-sphere interaction is represented by the sphere of a uniform radius 2R. The interaction potential b( q) is approximately given
8
Kajiwara and Miyamoto
by the Gaussian function when the interaction is softer [22,23], and Eq. (16) is rewritten as SI ðqÞc
1 1 þ 2A2 Mw c exp n2 q2
ð18Þ
where the Gaussian-type interaction potential is specified by the correlation length n of interaction.
C. Fundamentals of Nuclear Magnetic Resonance Spectroscopy Applied to the Conformational Analysis Nuclear magnetic resonance (NMR) spectroscopy has been widely employed in the structural analysis and the conformational dynamics of polymers in solution, gel, or solid states. However, its application is limited to the polymers that are not entirely crystalline in general. It provides information on microscopic chemical structures, including the primary structure, stereoregularity, conformation, and secondary structure of synthetic polymers, proteins, and polysaccharides. Various NMR techniques have also been developed to investigate molecular motion through relaxation times, correlation times, and self-diffusion coefficients. One of the advantages of NMR in the structure analysis is its sensitivity to a microscopic structure within a short-range order in comparison with smallangle x-ray scattering. The other advantages of NMR are that (1) it is a noninvasive method where no probes are needed; (2) the sample for measurement can be liquid, solid, or gel; (3) the NMR signals can be assigned individually to the main chain, the side chain, or the functional group of a sample and yield the structural information on a specific site; and (4) the molecular motion and dynamic structure (time-dependent structure) can be observed. However, NMR has some disadvantages: (1) the spatial position of atomic groups is not determined accurately; (2) the information on the long-range and higher-order structure will be lost; and (3) the duration time is long to observe NMR peaks from polymer samples with a reasonable S/N ratio and high resolution. Thus NMR spectroscopy compliments other methods of the structural and conformational analysis of polymers, including x-ray diffraction, light scattering, and small-angle x-ray (neutron) scattering. A variety of NMR techniques are available for the structure analysis of oligosaccharides and polysaccharides. The one-dimensional pulse NMR technique is mainly applied for the analysis of the saccharide primary structure in solution state and the determination of relaxation times. The solid state, high-resolution NIVIR technique can be applied for the structure analysis of oligosaccharides and polysaccharides in viscose solution, gel, and solid state. The two- or three-dimensional techniques are used to determine the primary and secondary structures and the conformation of oligosaccharides and polysaccharides. 1. Chemical Shift Oligosaccharides and polysaccharides show several 1H NMR signal peaks in the spectrum region between 2 and
6 ppm for protons on the ring. The anomeric protons (Hi) have peaks in the region between 4.5 and 5.5 ppm, whereas the chemical shifts for other protons (H2–H6) ranges from 2 to 4.5 ppm. The H1 chemical shift database will provide a starting key to assign the chemical shifts of unknown samples, although the chemical shift database for oligosaccharides and polysaccharides are still far from completion with respect to the accumulation and systematization. As the chemical shifts are also sensitive to the conformational change, solvent, and temperature, it requires experience and skill to identify the 1H NMR peaks for unknown oligosaccharides and polysaccharide samples. Various two-dimensional NMR techniques have been developed to facilitate the assignment and identification of the chemical shifts as described in a later section. The 1H NMR chemical shift data are summarized for monosaccharides in Table 3 [24]. The data are shown for monosaccharides as the components of oligosaccharides in which each is linked to an adjacent monosaccharide via a glycosidic bond oriented either below (a) or above (b) the plane of the ring. The chemical shift values of monosaccharides will assist the identification of oligosaccharides and polysaccharides, but the values vary considerably with the configuration and conformation of samples. 2. Relaxation Time The spin-lattice relaxation time (T1) and the spin–spin relaxation time (T2) reflect the conformational change and the local tumbling motion of oligosaccharides and polysaccharide chains. The relaxation process has been observed to understand the structure-dependent molecular motion, the helix-coil transition, the sol–gel transition, the crystalline structure, the amorphous structure, the aggregation structure, and the hydration structure. The spin-lattice relaxation time T1 is measured with the repeated p–s–2/p radio frequency (RF) pulse sequence by the inversion recovery method [25]. T1 follows Eq. (19) derived from Bloch’s equation: lnðAl As Þ ¼ ln 2Al s=T1
ð19Þ
where Al and As are the magnitude of the recovering vector of magnetization evolved by a p/2 RF pulse at time t = l and s, respectively. T1 is evaluated from the plot of ln(Al As) against s. T1 is given in terms of the viscosity g and temperature T [26] as 1 ¼ T1
128p3 h2
l4 a3 g
kT r6
ð20Þ
where l denotes a nuclear moment, a is the effective radius of a spherical molecule, and r is the distance from the observed nucleus to its magnetic neighbor. T1 decreases in proportion to g/T and a3 increases with r6. The effective volume a3 is replaced with the molar volume in the case of oligosaccharides and polysaccharides in solution. T1 as a function of the correlation time indicates the degree of molecular motion, and T1 takes a minimum at the temperature when the relaxation occurs according to the dipole–
Progress in Structural Characterization of Functional Polysaccharides
9
Table 3 Chemical Shifts (ppm) of Monosaccharides from Acetone at 2.225 ppm in D2O at 22–27jC Protons Monosaccharidea
H1
H2
H3
H4
H5
H6
H7
CH3
NAC
a-D-Glc-(1! h-D-Glc-(1! a-D-Man-(1! h-D-Man-(1! a-D-Gal-(1! h-D-Gal-(1! h-D-GlcNAc-(1! a-D-GalNAc-(1! h-D-GalNAc-(1! a-L-Fuc-(1! a-L-Rha-(1! h-D-Xyl-(1! 3-u-Me-a-L-Fuc-(1! 3-u-Me-a-L-Rha-(1! 2,3-di-u-Me-a-L-Rha-(1! 3,6-di-u-Me-h-D-Glc-(1!
5.1 4.4 1.9 4.7 5.2 4.5 4.7 5.2 4.7 5.1 4.9 4.5 4.8 5.0 5.1 4.7
3.56 3.31 3.98 4.04 3.84 3.52 3.75 4.24 3.96 3.69 4.06 3.27 3.70 4.24 3.94 3.34
3.72 3.51 3.83 3.63 3.90 3.67 3.56 3.92 3.87 3.90 3.80 3.43 3.40 3.59 3.52 3.31
3.42 3.41 3.70 3.58 4.02 3.92 3.48 4.00 3.92 3.79 3.46 3.61 – 3.52 3.41 3.51
3.77 3.45 3.70 3.37 4.34 3.71 3.45 4.07 3.65 4.1–4.9b 3.74
3.77 3.74 3.78 3.76 3.69 3.78 3.90 3.79 3.80 – – – – – – 3.66
3.87 3.92 3.89 3.93 3.71 3.75 3.67 3.68 3.75 – – – – – – 3.78
– – – – – – – – 1.23 1.28 – 1.32 1.32 1.32 –
– – – – – – 2.04 2.04 2.01 – – – – – – –
c
3.89 3.77 3.73 3.51
a These are average values for nonreducing terminal sugars linked by a glycosidic linkage to the adjacent monosaccharides. Signals for protons at the ring carbons are shifted downfield when linked by another monosaccharide at the hydroxyl group of that carbon. b These signals considerably vary more than other signals due to conformational features. c H5ax 3.29; H5eq 3.93. Source: From Ref. 24.
dipole interaction [27]. The correlation time, sc, is given approximately by sc ¼ 4p3 a3 g=3kT
ð21Þ
1
H T1 varies with the spin diffusion [28] and the value of T1 is much influenced by O2 gas. The T2 experiments are performed to observe the molecular motion in an extreme narrowing condition [27] where the viscosity of a sample solution is low and the motion is fast. The T2 measurements are suitable especially for 1H nuclei because the problem resulting from the spin diffusion can be avoided in the T2 experiments. The T2 value is determined by the Carr–Purcell [29]/Meiboom– Gill [30] (CPMG) method. Here the pulse sequence (p/2)– s–py–2s–py–2s–py–p. . .. (s is the pulse interval) is used to avoid the cumulative error due to incorrect pulse lengths. 3. High-Resolution Solid State Nuclear Magnetic Resonance A rapid isotropic tumbling molecular motion is restrained in the viscose solution state or in the solid state of oligosaccharides and polysaccharides. The NMR spectrum shows a proton dipolar broadening of many kilohertz due to strong dipole–dipole interaction and a chemical shift anisotropy as a result of the restraint of the molecular motion. A high-power, proton-decoupling field [31] is found to be effective to remove a proton dipolar broadening. 13C–1H scalar coupling can be removed by the high-
power proton dipolar decoupling (DD) to improve the resolution. A magic angle spinning (MAS) method is employed to diminish the chemical shift anisotropy [32]. A sample placed in a cylindrical rotor is rotated about an axis making an angle a with the magnetic field, H0, at 800–5000 Hz by air. The chemical shift Hamiltonian is composed of a timeindependent term and a time-dependent term [33]. The time-dependent term yields side bands at the multiples of the rotation rate in the spectrum, but the side bands disappear at a spinning rate faster than a half of the width of the chemical shift anisotropy powder pattern observed in the viscose solution or solid samples. When the sample is rotated at the fixed angle a being equal to 54.74j (magic angle) with respect to the magnetic field, the chemical shift anisotropy vanishes and the time-independent term contains only the isotropic chemical shift. Due to long 13C T1, a long repetition time is needed to observe an NMR spectrum with a sufficient S/N ratio and a high resolution in solid state experiments. The reduction of T1 can be achieved by transferring the energy of 13C spins in the excited state (at a high-spin temperature) to the NMR lattice. The energy is transferred from 13C spins at a highspin temperature to 1H spins in the cross-polarization (CP) technique [34,35] where the Hartmann–Hahn condition is satisfied. The RF pulse sequence of the CP technique for measuring 13C nuclei is shown in Fig. 6a. SL denotes a pulse for spin locking and DD is a pulse for heteronuclear dipolar decoupling. The Hartmann–Hahn condition is
10
Figure 6 Timing diagrams for the NMR pulse sequence: (a) CP, (b) COSY, (c) HOHAHA, and (d) NOESY.
satisfied by the pulse applied to 13C while applying the SL pulse. The signal created by CP is four times the original magnetization in an ideal condition. The DD and the MAS are usually combined with the CP technique to obtain highresolution spectra (CP/MAS). 4. Two-Dimensional Nuclear Magnetic Resonance In interpreting the NMR spectra, the first step is to identify signal peaks. As mentioned above, the spectra for oligosaccharides and polysaccharides are complicated and twodimensional (2-D) NMR technique is commonly applied to separate the NMR signals on the basis of J coupling. The 2D NMR technique yields information on the spin–spin coupling between heteronuclei, chemical exchange, and the nuclear Overhauser effect (NOE). The 2-D NMR technique involves several spectroscopic methods classified by the mode of pulse sequence (Fig. 6). The response of the nuclear spin system to the RF pulse is observed as FID (free induction decay) as a function of a time t2, which is Fourier transformed to yield an NMR spectrum in the conventional (1-D) spectroscopy. By applying two RF pulses with a time interval t1, a second time axis t1 (an evolution time) can be introduced where the
Kajiwara and Miyamoto
response of the nuclear spin system becomes a two-dimensional function of two independent times t1 and t2. When FID is two-dimensionally Fourier-transformed, a twodimensional spectroscopy is obtained as a function of two independent frequencies. The 2-D shift correlated spectroscopy (COSY) informs the connection of nuclei. The pulse sequence of COSY for 1H nuclei is shown in Fig. 6b. (p/2)/1 and (p/2)/2 are the first and second pulses, which differ in phase. The time interval between two pulses, t1, is an evolution time and t2 corresponds to an acquisition time. A 1H–1H COSY spectrum is represented by a square, where both axes correspond to 1H chemical shifts. The signals in the spectrum are classified in diagonal peaks and crosspeaks. The diagonal peaks are equivalent to the 1-D NMR spectroscopy. The cross-peaks appear symmetrically withrespect to the diagonal peaks and correspond to the difference of the chemical shifts of two sites specified on the diagonal line by the two coordinates of respective peak position. The 2-D homonuclear Hartman–Hahn spectroscopy (HOHAHA) reveals a spin–spin interaction network as a totally correlated spectroscopy that is obtained by changing the duration of the spin-locking application [36]. When the Hartman–Hahn condition is satisfied by spin locking, the magnetization transfer takes place by the spin–spin coupling between I and S spins and its degree can be adjusted by the duration of spin locking. Homonuclear Hartman–Hahn spectroscopy is more sensitive than COSY with respect to the line resolution, and facilitates the assignment of 1H signals along covalent bonds. To satisfy the Hartman–Hahn condition over a wide range, a proton broadband decoupling is introduced by a specially designed pulse sequence. Fig. 6c shows the pulse sequence of HOHAHA, where SLy is a spin-locking pulse and sm a mixing time. The MALEV-17 composite pulse [37] applied during the mixing time to lock spins over a wide frequency range. The nuclear Overhauser effect correlated spectroscopy (NOESY) observes the nuclear Overhauser effect due to the magnetic dipole–dipole interaction between nuclei in a short distance, and reveals the conformation, configuration, and chemical exchange of large molecules [38]. The pulse sequence of NOESY is basically the same as COSY except for the additional p/2 pulse after a fixed time sm as shown in Fig. 6d, where sm denotes a mixing time. The distance between 1H nuclei is determined from the intensity of cross-peaks, and offers a mean of investigating spatial relationships between nuclei through NOE. The crossrelaxation rate for an I and S spin system, rIS, is a function of the distance between the I and S spin: c4 t2 rIS ¼ 10r6
6sc sc 1 þ 4x2 s2c
ð22Þ
where x is the Larmor frequency and the sc is the correlation time of reorientation [39]. rIS is evaluated from the sm dependence of cross-peak intensities. The spatial information obtained by NOESY is restricted within the distance of
Progress in Structural Characterization of Functional Polysaccharides
about 0.5 nm. sc depends on the motility of molecules. The cross-peaks show negative and positive values for xsc < 1 and xsc > 1, respectively. When xsc c 1, the cross-peaks of NOE are not observed. By applying spin locking, a positive NOB is observed over the wide time scale of molecular motion. The rotating frame nuclear Overhauser effect spectroscopy (ROESY) is developed [39,40] to observe NOB of the sample whose molecular weight ranges from 1000 to 2000 and xsc c 1.
D. Molecular Modeling 1. Monte Carlo Method Two dihedral angles / and w with respect to the glycosidic bond determine the conformation of a disaccharide, provided that a pyranose ring is rigid (Fig. 7). The conformational analysis of a disaccharide thus comprises the
11
evaluation of a total conformational energy as a function of a pair / and w. / and w can take any value between 180j and +180j. The most likely conformation is expected to have the lowest potential energy. For example, 38 pairs of / and w evaluated from the crystallographic data of maltose Glcpa 1!4 Glc are found to lay within the low-energy range of 2 kcal/mol above the absolute energy minimum on the energy map provided by molecular mechanical calculation, proving the validity of computer modeling. Here molecular modeling permits to evaluate the range of attainable conformations in terms of the potential energy at each point specified by a pair of / and w. The observed value of / and w will vary among the attainable conformations according to the crystal packing (in the solid state) or the type of solvent (in the solution). Fig. 7 shows the conformational energy map of maltose, cellobiose, xylobiose, chitobiose, laminaribiose, and sphorobiose calculated by
Figure 7 Definition of two dihedral angles, / and w, to determine the conformation of a disaccharide, and 2-D contour energy map (the potential energy as a function of two dihedral angles / and w) of (a) maltose, (b) cellobiose, (c) xylobiose, (d) chitobiose, (e) laminaribiose (s = 112.5j), and (f ) sophorose.
Figure 7 Continued.
Progress in Structural Characterization of Functional Polysaccharides
13
determined by a set of / and w when the bond angle s is fixed. The effect of excluded volume can be taken into account by excluding the step that places a unit in a specified vicinity of the space occupied already by the unit in a previous step. Because the polysaccharide chain undergoes thermal fluctuation in solution, the scattering from the solution is observed as an average over space and time. Assuming the ergodicity, several chains are independently generated to constitute a microcanonical ensemble, and the particle scattering function is then given by an ensemble average over the scattering calculated from the atomic coordinates of each generated chain according to Eq. (12). Fig. 9 shows the scattering profiles averaged over 500 chains of two 1,4glucans, (1!4)-a-D-glucan (amylose), and (1!4)-h-D-glucan (cellulose), generated by the scheme represented by Fig. 8 with varying the number of glucosidic residues in terms of the Kratky plots by plotting q2I( q) against q. Here the occurrence probability for a pair of / and w is provided by
Figure 7 Continued.
molecular mechanics (MM2 or MM3) with the force-field including bond vibration, bond stretching, angular torsion, and van der Waals interaction (see Table 1 for the terminology). Here the glucose residue is assumed to be rigid and replaced with a virtual bond connecting the neighboring oxygen atoms of the glycosidic linkage (Fig. 7). The bond angle s is fixed, for example, to 110j in the case of amylose so as to yield a consistent value for the radius of gyration as observed for high molecular weight amylose. Longer chains are generated by the Monte Carlo method according to the scheme summarized in Fig. 8, where the assumption is made that the short-range interaction between two adjacent residues determines the range of permissible values of a pair of the dihedral angles / and w. That is, a pair of / and w is provided from the energy map (Fig. 7) according to the occurrence probability P(/, w) specified by the Boltzmann factor associated with the potential energy E(/, w) of a disaccharide with a set of / and w. Here P(/, w) is given as Pð/; wÞ ¼ c exp½Eð/; wÞ=kB T
ð23Þ
with kB being a Boltzmann constant, T an absolute temperature, and c a normalization constant. A chain is constructed step by step as the geometry of each unit is
Figure 8 Flow chart to generate polysaccharide chains and calculate the scattering factor.
14
Kajiwara and Miyamoto
Figure 9 Simulated scattering profiles of (1!4)-h-D-glucan (a) and (1!4)-h-D-glucan (b) as a function of the number of glucosidic residues with snapshots of a simulated structure of respective glucan chains composed of 40 glucosidic residues (a stereo figure) on the right.
the energy map of Fig. 7. The snapshots of simulated chains (DP = 40) are also shown on the right side of the Kratky plots. The simulated amylose chain reveals the wobble helical conformation with localized highly ordered helical regions, whereas the cellulose chain seems to have a rather extended chain structure as expected from the primary structure. The calculated scattering profiles reveal a pronounced peak in Kratky plots at q = 0.2 A˚1 for (1!4)-aD-glucan of higher degrees of polymerization, whereas (1!4)-h-D-glucan exhibits a scattering profile typical to a rigid rod-like molecule. The intramolecular hydrogen bonding is responsible for stabilizing the quasi-helical
chain conformation of (1!4)-a-D-glucan, which yields a thicker cross-sectional radius of gyration evaluated as approximately 5 A˚ from the cross-sectional Guinier plot [Eq. (6)] of the simulated scattering profiles for (1!4)-a-Dglucan chains of over 20 glucosidic residues. The crosssectional radius of gyration remains as small as 2.1 A˚ in the case of (1!4)-h-D-glucan chains, whose extended chain conformation promotes to assume the intermolecular hydrogen bonding to form non-water-soluble aggregates. Table 4 summarizes the radius of gyration of (1!4)-a-Dglucan and (1!4)-h-D-glucan, each calculated from the simulated profiles and/or estimated from the observed
Progress in Structural Characterization of Functional Polysaccharides
15
SAXS profiles. Although some refinement of the probability map is necessary, the simulation accounts, at least qualitatively, for the DP dependence of the radius of gyration and the difference in the radius of gyration due to the glucosidic linkage mode. When the saccharide chain is longer, the excluded volume effect becomes more serious. The excluded volume effect can be taken into account by considering the interaction between the nonbonded units. Conventionally, the repulsive interaction is dealt with in the Monte Carlo simulation by replacing the chain units (segments) with hard spheres of a finite radius. Fig. 10 demonstrates the snapshots of amylose chain generated by the Monte Carlo method with and without excluded volume, which is represented by a sphere of a radius 4 A˚ at the position of each glycosidic oxygen. The excluded volume effect is seen to expand the chain, but the helical nature of amylosic chains is retained in both unperturbed and perturbed states. 2. Molecular Dynamics The Monte Carlo method described in the preceding section is based on the disaccharide conformation energy map, and no water molecules are taken into account in the model. Although the Monte Carlo method is capable of simulating longer polysaccharide chains, it does not allow including the solvation effect directly through water-mediated hydrogen bonds. Molecular dynamics (MD) simulations [41] can be applied to the structural studies of various polysaccharides, where water molecules can be explicitly included in the simulation. However, the MD simulation is restricted to relatively shorter chains owing to a present computational capacity. The results of the MD simulation depend on the employed force-filled models such as Gromos [42], Glycam93/99 [43], and Cff91/Cff [44], as well as on the starting conformation. Among the force fields mentioned above, Gromos and Glycam is composed of a set of parameters specifically developed for amylose; however, they differ in the treatment of the exoanomeric effect
Table 4 Radius of Gyration of (1!4)-a-D-Glucan and (1!4)-h-D-Glucan Oligomers DP 1 2 3 4 5 6 7 8 9 10 20 40 50
(1!4)-h-D-glucan (A˚) (obs.) (cal.) 3.53 4.85 6.22 7.61 9.00 10.40 11.84 13.23 14.70 28.53 55.18
(1!4)-a-D-glucan (A˚) (obs.) (cal.) 3.47
–
4.55 5.28 6.15 6.69 7.26 8.08 10.21 10.11
4.43 5.32 6.04 6.56 7.06 7.54 7.77 8.83 13.89 23.18 28.12
Figure 10 Snapshots of amylose chain generated by the Monte Carlo method with (b) and without (a) excluded volume. Here the excluded volume is taken into account by replacing the glycosidic oxygen (denoted by a circle in the Figure) with the hard sphere of radius 4 A˚.
on the glycosidic linkages. Here Gromos ignores the exoanomeric effect, while Glycam incorporates the effect through the torsional terms determined from the ab initio geometry optimization at the HF 6-31G* level. Cff91 is a general-purpose force field for biomolecules, and Cff is expanded from Cff91 to include the parameters with a proper account of the anomeric effect on the glycosidic linkages. The example of the MD simulations will be shown in the later section.
III. STRUCTURAL AND CONFORMATIONAL ANALYSIS OF OLIGOSACCHARIDES AND POLYSACCHARIDES The structural characterization of simple homoglucans is mainly introduced in this section. The structural and mechanical properties of the gels from various marine polysaccharides, plant polysaccharides, microbial polysaccharides, and animal polysaccharides are reviewed by Clark and Ross-Murphy [45]. This chapter intends to demonstrate the advanced methods applied for the structural and conformational characterization of oligosaccharides and polysaccharides, particularly in solution, by taking the examples of the homoglucans composed of different modes of glucosidic linkage.
16
A. (1!4)-A-D-Glucan Represented by Amylose The oligomers of (1!4)-a-D-glucans dissolve well in water. The observed SAXS profiles from maltohexaose and maltooctaose are shown in Fig. 11, where no effect of association was observed. The simulated SAXS profiles are also shown in Fig. 11 to examine the consistency of simulation with the observed profiles. The characteristics of wobbled helix represented by a pronounced peak in the Kratky plots become more distinct in maltooctaose than in maltohexaose as expected from the molecular weight dependence of simulated SAXS profiles (Fig. 9). A good agreement between simulated and observed SAXS profiles assures that the simulation can be extended to a longer chain to elucidate
Kajiwara and Miyamoto
a single chain conformation of amylose. Here no adjustable parameter is involved, except for the normalization with respect to the scattered intensity at q = 0. Amylose is known to assume a double-stranded (Bform) [46,47] or single-stranded helical (V-form) [48] conformation in a solid state from the analysis of the x-ray fiber diffraction, the x-ray powder, and the electron diffraction pattern of single crystals. Amylose aqueous solution forms gel by cooling. Gelation takes place through the formation of nanocrystallites that serve as cross-linking domains. Particle scattering from model nanocrystallites is calculated [49] by assuming nanocrystallites composed of B-form double helices or single-stranded V helices. The model nanocrystallite is approximately represented by an
Figure 11 Simulated and observed scattering profiles from maltohexaose (a) and maltooctaose (b). The Figures on the right show a snapshot conformation of simulated maltohexaose and maltooctaose, respectively (a stereoview).
Progress in Structural Characterization of Functional Polysaccharides
elliptical cylinder of 8.32-nm thickness (contains 42–222 duplexes composed of 24 glucosidic residues per strand) or a parallelepiped of 6.44-nm thickness (contains 120 helices composed of 24 glucosidic residues per strand) for the Bform or the V-form, respectively. The SAXS profile from amylose aqueous solution reveals a sharp upturn at q!0 in the Kratky plots (Fig. 12) [ln q2I( q) plotted against q] according to the sol–gel transition. This pronounced upturn is ascribed on the formation of an infinite structure (gel) as expected by the cascade theory of gelation [50]. At higher q regions, two scattering profiles from sol and gel coincide, indicating that the local conformation is identical in the sol and gel states. The local conformation is probably represented by a singlestranded chain simulated by the Monte Carlo method shown in Fig. 9a, considering that single-stranded chains are present in amorphous region of gel or in solution [51]. The observed profiles are fit to the scattering profile from
Figure 12 Small-angle x-ray scattering profile from amylose gel and sol, where closed and open circles denote gel and sol, respectively. Solid lines represent the calculated scattering profile from simulated (1!4)-h-D-glucan chains of DP = 40.
17
Figure 13 Scattering profile of amylose gel decomposed into two components. Iexcess denotes the excess scattering from amylose gel with respect to amylose sol (= IGEL ISOL). Imodel is the scattering calculated from the oblate ellipsoid of revolution (12.9 13.1 4.3 nm), and Ical = ISOL + Imodel.
simulated (1!4)-a-D-glucan chains (DP = 40) in Fig. 12. The Guinier plots for the cross section [Eq. (6)] yields the cross-sectional radius of gyration as 0.45 nm in both gel and sol. The value of 0.45 nm (close to 0.5 nm), which is evaluated for the cross-sectional radius of gyration from the model double-stranded helix [52], also corresponds to an apparent cross-sectional radius of gyration of a single (1!4)-a-D-glucan chain. Here the deviation at lower q ranges is considered to be due to the presence of doublestranded helices formed by the coupling of two neighboring single-stranded helices without significantly disturbing the conformation. The SAXS profile from amylose gel was analyzed in terms of two components representing nanocrystallites and amorphous region [53], respectively, by assuming that no interference would take place between two components. The structure of the amorphous region in amylose gel should be identical to that in the sol state. Thus the excess scattering in the gel state with respect to the sol state mainly resulted from the formation of nanocrystallites that function as the cross-linking domain ( junction zone). The oblate ellipsoid of revolution was found to yield the scattering profile fit to the excess scattering (Fig. 13), and its dimension (three semiaxes 12.9 13.1 4–3 nm) approximately corresponds to the nanocrystallite composed of 42 B-form duplexes with 24 glucosidic residues per strand. The molecular dynamics simulation was performed on maltopentaose with currently available force fields [54]. The results are compared with the small-angle x-ray scattering observed from maltopentaose in aqueous solution. Fig. 14 compares the simulated profiles with the observed SAXS profiles, where Fig. 14a provides a series of results simulated with available force fields, and Fig. 14b the
18
Kajiwara and Miyamoto
B. (1!4)-B-D-Glucan Represented by Cellulose
Figure 14 Small-angle x-ray scattering profiles observed from maltopentaose aqueous solution (open circles) of 20.13 mg/mL at 25jC with simulated profiles (respective curves). (a) MD results (the radius gyration and force field are shown in the Figure) and (b) Monte Carlo results and profiles calculated from crystalline regular helices (the radius of gyration and the source of other data are shown in the Figure).
Monte Carlo results with two probability maps (Monte Carlo K denotes a rigid map employed in Fig. 9a) and the profiles calculated from the atomic coordinates of three regular helices. Both Monte Carlo results show a satisfactory agreement with observed SAXS profiles, where a small difference due to the glucose geometry was observed at higher q. The results of MD simulations vary with the force fields, and the Cff91 seems to yield the best fit to an observed profile. Because the helix model of Goldsmith et al. [55] fits satisfactorily well to the observed SAXS profile, maltopentaose seems to assume a quasi-helical conformation specified by a radius of 5.38 A˚, a rise of 2.44 A˚, a pitch of 17.60 A˚, a repeat of 7.2 A˚, / = 105j, and w = 135j. A typical conformation of maltopentaose is shown in Fig. 15 as simulated with various force fields. In fact, the conformation observed by the MS simulation with the Cff91 is similar to the helix model of Goldsmith et al.
Cellopentaose cannot be completely dissolved in water because of a strong intermolecular interaction by hydrogen bonding through OH groups on C6. The SAXS from the aqueous solution of cellopentaose (30 mg/mL) exhibits a sharp upturn toward lower q due to the formation of large aggregates (Fig. 16). If the aggregation is caused by intermolecular hydrogen bonding, the aggregates are considered to be formed by the side-by-side stacking of cellopentaose chains. The simulated profile (a solid line in Fig. 16) reflects a chain stiffness of a (1!4)-h-D-glucan chain, but the observed profile significantly deviates from the simulated profile at a lower q region. The cross-sectional radius of gyration is estimated as 3.5 A˚ at the intermediate q range and as over 70 A˚ at the smaller q range. A single (1!4)-h-D-glucan chain has the cross-sectional radius of gyration of 2.1 A˚, so that two cellopentaose chains are considered to form a stable aggregate and some further aggregate into a larger cluster. The intermolecular hydrogen bonds can be broken by adding urea in the aqueous solution of cellopentaose. Fig. 16b observes a good agreement between the observed and simulated SAXS profiles, and the cross-sectional radius of gyration is estimated as 2.1 A˚, which is expected for a single (1!4)-A˚-D-glucan chain. Regarding the local conformation of (1!4)-h-D-glucan chain in the presence of water, the potential use of multiple-RELAY-COSY is suggested from the analysis of complex spin networks of 1H NMR spectra of cellooligosaccharides where the complete assignment of 1H NMR resonance was achieved for cellotriose [56]. Solventsuppression COSY provides also a useful method to elucidate the interaction of the hydroxyl groups with water [57]. The 1H NMR of methyl h-cellobioside in H2O-acetoned6 (85 :15) yields sharp signals due to the seven hydroxyl groups at 20jC (Fig. 17), where all signals are identified [57].
Figure 15 Stereoviews of the snapshot conformations of maltopentaose as simulated by the Monte Carlo method and MD, including regular amylose helices. (a) Regular helix (8.3 A˚) [47], (b) regular helix (7.4 A˚) [55], (c) regular helix (5.9 A˚) [48], (d) Monte Carlo/MM3 (7.57 A˚), (e) Glycam93 (8.85 A˚), (f ) Glycam99 (8.08 A˚), (g) modified Glycam93 (7.72 A˚), (h) Cff91 (7.83 A˚), (i) Cff (8.30 A˚), ( j ) Gromos (8.32 A˚). The values in each bracket denote the radius of gyration, which was evaluated as 7.4 F 0.2 A˚ from the SAXS profile.
Progress in Structural Characterization of Functional Polysaccharides
19
Figure 16 Small-angle x-ray scattering profile from cellopentaose in water (a) and in 1 M urea aqueous solution (observed and simulated as indicated in the Figures). A stereoview of a simulated cellopentaose chain is shown on the right.
The crystal structure of cellulose has been a subject of a long-standing argument. Cellulose is known to have four different polymorphic crystalline forms classified as cellulose I, II, III, and IV. Parallel chain packing is proposed for native cellulose I [58], and regenerated cellulose II is supposed to assume antiparallel chain packing [59,60] as analyzed from the results of x-ray fiber diffraction pattern. Because CP/MAS 13C NMR revealed cellulose I as being composed of the allomorphic mixture of triclinic Ia and monoclinic Ih, the refinement of cellulose crystal structure again became a main issue in the cellulose science [61]. Here the multiplicity at C4, C1, or C6 is due to magnetically nonequivalent sites present in crystalline domain, and is
found to vary its pattern, implying that the ratio of two allomorphs Ia/Ih differs by the origin of native cellulose [62–64]. It is interesting to note that a single microfibril of native cellulose is a composite of two crystalline phases, Ia and Ih [65,66]. The crystal structure of cellulose II is considered to consist of two antiparallel chains of almost identical conformation packed in a monoclinic unit cell, where the hydroxymethyl group at C6 assumes a tg or a gt conformation in the ‘‘up’’ or ‘‘down’’ chain, respectively. However, CP/MAS 13C NMR exhibits a singlet at 64 ppm for the C6 resonance from cellulose II polymorph against the expected doublet to be observed at 64 and 66 ppm from the
20
Kajiwara and Miyamoto
tg and gt conformations [67]. The cellulose II crystal structure is re-examined [68] from the crystal structure of cellodextrin oligomers, including h-D-cellotetraose (Fig. 18) [69,70] and methyl h-cellotrio side [71]. In those cellodextrin oligomers, all the hydroxymethyl groups (C6–O6 bonds) are in the gt position, but the two antiparallel chains assume a different glucose ring conformation. This finding accounts, at least qualitatively, a singlet for C6 and a doublet for C1 and C4 observed for cellulose II by CP/ MAS 13C NMR.
C. (1!3)-B-D-Glucan
Figure 17 1H NMR spectra of methyl h-cellobioside in H2O–acetone–d6 (85:15) at 20jC.
Figure 18
(1!3)-h-D-glucan consists of a backbone of a group of extracellular plant/fungal glucans such as cinerean, curdlan, krestin, laminaran, lentinan, schizophyllan, and scleroglucan, which are known to affect the immune system as an unspecific modulator [72]. Except for curdlan, which is linear (1!3)-h-D-glucan, the (1!3)-h-D-glucan family contains some amount of h(1!6) branched Dglucose residues, and assumes a triple-helical conformation. Although the structural requirement is not explicitly understood, the antitumor activity is said to be more
Molecular structure (stereoview) of two h-D-cellotetraose chains.
Progress in Structural Characterization of Functional Polysaccharides
pronounced in lower h(1!6) branched (1!3)-h-D-glucans with a relatively high molecular mass [73]. Those (1!3)-hD-glucans form triple-stranded helices of high rigidity in aqueous solution [74,75], and the TEM image revealed the macrocyclic species made of multiple triple-stranded (1!3)-h-D-glucan chains in some cases after a cycle of denaturation-renaturation process [76]. Laminaran is produced by Laminaria seaweeds, and contains a small amount of h(1!6)-branched D-glucose residues and alkyl groups at reductive ends. The conformation of laminara oligosaccharides was characterized in aqueous solution by the combined method of small-angle x-ray scattering and Monte Carlo simulation [77]. The conformational energy map of laminarabiose (Fig. 7e) shows four local minima including two global minima around (/, w) = (0j, 50j) and (/, w) = (30j, 0j). The crystallographic data of laminarabiose and laminarabioside derivatives (except for methyl b-D-laminarabioside and h-D-laminarabiose) confirm that two dihedral angles / and w with respect to the glycosidic bond fall in one of the global minima in the conformational energy map of laminarabiose (see Table 2). w is twisted by the formation of intramolecular hydrogen bond between O4V and O5, which is prevented by introducing acetate substituents. The global minima indicate the helical conformation of laminaran, which will be interrupted by the other local minima at (20j, 170j) and (160j, 10j). Over 500 chains were generated to constitute a statistical ensemble of laminara-oligomers according to the scheme shown in Fig. 8, and the average scattering factor
Figure 19
21
over the ensemble was calculated to compare with the observed SAXS profiles. The simulated scattering profiles (in terms of the Kratky plots) exhibit characteristic maxima of helical conformation with increasing degree of polymerization (Fig. 19). Fig. 20 shows the observed and calculated SAXS profiles of laminarahexaose together with a snapshot of a simulated chain. Although laminarahexaose is not long enough to show the characteristics of helical conformation, the observed SAXS profile is in good agreement with the simulated scattering profile. The observed profile has a smooth shoulder at q = 0.2–0.25 A˚1, whereas a simulated profile shows a slight peak at q = 0.2 A˚1 due to a quasi-helical structure. The deviation of the observed profile from the simulated one is probably due to hydration, which is not properly taken into account in the simulation. The radius of gyration RG and the crosssectional radius of gyration RG,c are consistent with the respective values evaluated from observed and simulated profiles—7.8 A˚ (RG) and 3.0 A˚ (RG,c) from the observed profile for laminarahexaose, and 7.7 A˚ (RG) and 3.4 A˚ (RG,c) from the simulation. A triple-helical structure has been proposed for (1!3)h-D-glucan [78,79]. For example, the molecular and crystal structure of the anhydrous curdlan and its hydrated form was determined by combined x-ray diffraction from oriented curdlan fibers and stereochemical model refinement [80]. Here both hydrous and anhydrous forms assume a right-handed triplex (sixfold triple-helical conformation) crystallized in a hexagonal unit cell with the interstrand O2: : : O2 hydrogen bonds. Curdlan is believed to assume a
Scattering profiles calculated for laminara-oligosaccharides as a function of the degree of polymerization.
22
Kajiwara and Miyamoto
Figure 20 Small-angle x-ray scattering profile from laminarahexaose in water (observed and simulated as indicated in the Figure). A stereoview of a simulated laminarahexaose chain is shown on the right.
single- or triple-helical sevenfold conformation by swelling, where a chain is expanded along the chain direction to increase the helix repeat distance to 22.7 A˚ from 17.6 A˚ (in anhydrous form) or 18.8 A˚ (in hydrous form). Regular or irregular short-branch substitutions on the main chain O6 hydroxyls seem not to affect the triplex structure as exemplified by scleroglucan [81], schizophyllan [75], and lentinan [82], which retain a triplex structure even in aqueous solution. It is interesting to note that the dihedral angles / and w of curdlan polymorphs are similar to those of the acetylated derivatives of laminarabiose or laminarabioside (Table 2). Similar / and w values are also evaluated from the molecular structure of the tetrasacharride (1!6) branched (1!3)-h-D-glucan [83].
Gel is formed in the aqueous solution of (1!3)-h-Dglucans, but its mechanism seems to differ from linear and branched species. Curdlan low-set gel is prepared by heating a slurry (>0.5% w/v) to above 60jC, and will be high-set with annealing at 95jC [84]. Gelation is suggested to proceed with breaking hydrogen bonds to solubilize curdlan and reforming intermolecular hydrogen bonds subsequently to consist the junction zones. Hydrophobic interaction promotes the intermolecular association of curdlan at elevated temperatures to form stronger highset gel. Thus curdlan gel is supposed to contain both liquid-like (composed of flexible chains) and solid-like (composed of associated chains) domains. 13C NMR was applied to curdlan gel where various methods (including
Progress in Structural Characterization of Functional Polysaccharides
CP/MAS, broadband coupling, and MAS) were employed to obtain the signals from the domains of different molecular motions [85]. Fig. 21 shows the 13C NMR spectra of curdlan hydrate and gel recorded by various methods. Here a conventional high-resolution NMR coupled with broadband decoupling confirms that the liquid-like domain is composed of single-helical chains that are flexible and undergo free molecular motion. The intermediate domain is also composed of single chains as indicated by high-power dipolar decoupling with magic angle spinning (MAS). The CP/MAS spectrum reveals a small amount of triple helices visible in the solid-like domain as shown by an arrow (a C5 signal from the triple helix) in Fig. 21, but otherwise gives the characteristics of the swollen sevenfold helical form of solid curdlan with C3 at 87 ppm and no peak at 79 ppm. Annealing at elevated temperatures results in the increase of the fraction of anhydrous (in a later stage hydrous) sixfold helical domains and the decrease of the swollen form portion [86]. The NMR observation indicates that curdlan undergoes gelation by forming quasi-crosslinking domain composed of single helical chains associated hydrophobically after swelling at lower temperatures, and subsequently, by increasing the triple-helical fraction at elevated temperatures. The triple-helical conformation
23
of the anhydrous form appears at the early stage of annealing, and eventually the transformation takes place from the anhydrous to the hydrous form. The 13C NMR of branched (1!3)-h-D-glucan gel such as lentinan and schizophyllan shows the characteristic peaks of the triple helix [87], but the peaks corresponding to the liquid-like domain disappear by gelation [82]. Thus the gelation of h(1!6) branched (1!3)-h-D-glucans is mainly due to partial association of triple-helical chains. The gelation of schizophyllan is promoted by the presence of sorbitol [88] where thermoreversible optically transparent gel is formed by lowering the temperature. However, the small-angle x-ray scattering (SAXS) profile from the schizophyllan/sorbitol system shows less-marked change by the sol–gel transition. The 1.5% aqueous solution of schizophyllan containing 4 M sorbitol is sol at 60jC but forms transparent gel at 5jC. The SAXS profiles from the solution at respective temperature were analyzed in terms of a modified broken rod model [89], which reads
q2 IðqÞc
X i
pqwi MLi
4J12 ðqRci Þ ðqRci Þ2
þ const:
ð24Þ
Figure 21 13C NMR spectra of curdlan hydrate (A) and gel (B–D), observed by CP/MAS (A, D), by broadband decoupling (B), and by MAS (C).
24
where wi, MLi, and Rci denote the weight fraction, the linear mass density, and the cross-sectional radius of the rod-like component i, respectively. J1(x) is the first-order Bessel function, and the constant term accounts that the rod-like components are connected by a free joint. The model takes into account the heterogeneity with respect to the cross-section. The results are shown in Fig. 22 in two types of Guinier plots. Schizophyllan assumes a triplehelical conformation in water, and undergoes no conformational change by decreasing the temperature from 60jC to 5jC as shown in Fig. 22a,b, where the scattering profile was calculated from the molecular model of schizophyllan triple helix. The cross-sectional radius of gyration of schizophyllan is estimated as 6.4 A˚. When sorbitol is added, the cross-sectional Guinier plots yield a smaller apparent cross-sectional radius (5.1 A˚), which becomes even smaller (4.6 A˚) by gel formation at a lower temperature (5jC). Here the SAXS scattering profile at 60jC was fitted with the molecular model of (1!3)-h-D-glucan triple helices with no side chain (i.e., curdlan-type triple helix). The SAXS profile at 5jC can be fitted by a modified
Kajiwara and Miyamoto
broken rod model [Eq. (24)] where each component is replaced with a triple helix and a single coil of the schizophyllan molecular model. The atomic radius is reduced to half of the van der Waals radius to account for the smaller cross-sectional radius. The inclusion of a constant term is necessary, so that schizophyllan triple helices are speculated to disentangle into single chains that act as a free joint. Sorbitol breaks intramolecular hydrogen bonds of schizophyllan triple helices, and solvates the broken parts to form a cross-linking junction by intermolecular hydrogen bonding through sorbitol. An apparent smaller atomic radius observed at 5jC is probably due to solvated sorbitol reducing the contrast between solvent and solute.
D. Cyclic and Linear (1!2)-B-D-Glucan Gram-negative bacteria such as Agrobacterium and Rhizobium [90,91] are known to produce a cyclic (1!2)-h-Dglucan referred to as cyclosophoran. The DP value (the
Figure 22 Small-angle x-ray scattering profiles from the 1.5% aqueous solution of schizophyllan and schizophyllan/4 M sorbitol at 60jC (a) and 5jC (b). The solid lines represent the scattering profiles calculated according to the molecular model (c) and Eq. (23).
Progress in Structural Characterization of Functional Polysaccharides
Figure 22
Continued.
25
degree of polymerization) of cyclosophoran varies from 17 to 24 depending on the bacterial strain; the largest DP reported is 40. Cyclosophoran is thought to act as a regulator of the osmotic balance between the cytoplasm and the periplasmic space for bacteria to adapt the change in environmental osmolality [92] or to mediate the bacterium–plant host [93] interactions during the infection of the host. Although the exact physiological role of cyclic (1!2)h-D-glucan is a matter of speculation, its physiological function is assumed to be closely related to its conformation [94]. The conformation of (1!2)-h-D-glucan has been extensively investigated by computer modeling and 13C/1H NMR [95], but the homopolymeric nature and conformational identity of the glucose residues obscure the structure determination by NMR. The conformation of cyclic and linear (1!2)-h-Dglucans was investigated by the combination of the Monte Carlo simulation and SAXS [96]. Cyclosophoran mixtures produced by Agrobacterium radiobactor and Rhizobium fphaseoli were fractionated into nine fractions from DP = 17 to 25 (each designated as CS17 to CS25) by highperformance liquid crystallography (HPLC). Linear (1!2)-h-D-glucans (designated as LS 19 and LS2 1 according to DP) was prepared by acid hydrolysis of CS21 and subsequent fractionation by HPLC. Small-angle x-ray scattering (SAXS) was observed from the aqueous solutions of cyclic glucans (CS17 to CS24) and linear glucans (LS19 and LS21) at 25jC where the concentration was varied from 10 to 40 mg/mL (for the cyclic glucans) or from 12.5 to 25 mg/mL (for the linear glucans). The observed range of the magnitude of the scattering vector was from q = 2.50 102 A˚1 to q = 0.375 A˚1, which is equivalent to the Bragg spacing from 251 to 16.8 A˚. The observed SAXS profiles reveal the structural difference of cyclic and linear (1!2)-h-D-glucan chains in aqueous solution in the region of q > 0.15 A˚1 (Fig. 23). The radius of gyration, RG, was evaluated from the initial slope of the Guinier plots as summarized in Table 5. The cross-sectional radius of gyration Rc was evaluated from the Guinier plots for cross section [Eq. (6)] in the case of linear (1!2)-h-D-glucan chains or the thickness T from the Guinier plots for thickness [Eq. (7)] in the case of cyclic (1!2)-h-D-glucan chains. The results indicate that a cyclic (1!2)-h-D-glucan chain assumes the shape of a flat disk and a linear homolog the shape of a cylinder. The compact conformation of a cyclic (1!2)-h-D-glucan chain is confirmed from the smaller radius of gyration in comparison with a corresponding linear (1!2)-h-D-glucan chain. (1!2)-h-D-glucan chains were generated by the Monte Carlo method, consistent with the disaccharide conformational energy map (Fig. 7f ). The region of the energy well is specified as the conformation +A for w > 20j, or A for w < 20j according to York [95]. The glucose residue is assumed to be rigid, and the conformational energy map for h-sophorobiose is calculated by the molecular mechanics as a function of the dihedral angles / and w defined as / = h[H1, C1, O, C2V] and w = h[C1, O, C2V, H2V]. Nonbonded van der Waals interactions and
26
Kajiwara and Miyamoto
Figure 23 Small-angle x-ray scattering profiles of cyclic and linear (1!2)-h-D-glucan chains in (a) Guinier plots [ln P( q) plotted against q2] and (b) Kratky plots [ q2P( q) plotted against q].
electrostatic interactions due to partial charges are taken into account in the calculation. The occurrence probability is given by the Boltzmann factor for a pair of (/, w) normalized with respect to the sum of the Boltzmann factors for all pairs of (/, w), whereas the bond angle s at the glycosidic oxygen is fixed at 113.6j. Among the chains generated by the Monte Carlo method, those with the end-to-end distance less than 1.5 A˚ are collected to compose an ensemble of cyclic (1!2)-h-D-glucan chains. An ensemble of linear (1!2)-h-D-glucan is composed of 500 chains.
The scattering factors are calculated according to Eq. (12) from the atomic coordinates of generated chains in an ensemble, with the radii of carbon and oxygen atoms being taken to be 1.67 and 1.50 A˚, respectively. Here all the O6 atoms of the glucose unit are affixed to the pyranose ring at a gauche–trans (gt) position with respect to the torsion angle h[O5, C5, C6, O6] and the torsion angle h[C4, C5, C6, O6], respectively. Fig. 24 shows a reasonable agreement of the simulated scattering profile for cyclic (1!2)-h-D-glucans with that observed by SAXS, where the scattering profiles calculated
Progress in Structural Characterization of Functional Polysaccharides Table 5 The Radius of Gyration RG, the Cross-Sectional Radius of Gyration Rc, and the Thickness T of Cyclic and Linear (1!2)-h-D-Glucan Chains Evaluated from the Corresponding Guinier Plots of SAXS Data Sample code
RG (A˚)
Rc (A˚)
T (A˚)
7.8 8.1 8.5 8.3 8.6 8.4 8.9 10.6 11.1 12.0
– – – – – – – – 5.9 6.6
10.0 10.0 10.0 10.0 10.5 10.7 10.8 9.8 – –
CS17 CS18 CS19 CS20 CS21 CS22 CS23 CS24 LS19 LS21
27
large molecule for the formation of an inclusion complex. All the glucosidic linkage torsion angles are found within the region A of the conformational energy map (Fig. 7f ) with 13 linkages in the region +A and 7 linkages in the region A where no special mode is observed for arranging +A and A. The Monte Carlo simulation for linear (1!2)-h-Dglucans yields less satisfactory results with respect to the scattering profile (Fig. 24). Although the Monte Carlo simulation yields a consistent value of the radius of gyration with an observed one, the deviation in the scattering profile becomes apparent at u (u qRG) > 1.3. A good linearity observed in the cross-sectional Guinier plots [Eq. (6)] indicates a cylindrical shape of a linear (1!2)-h-Dglucan chain as shown in Fig. 26 with space filling models. The cross-sectional diameter is evaluated as 11.8 A˚ (LS 19)
from two elementary models (a rigid ring [97] and a flexible Gaussian ring [98]) are shown for comparison. The particle scattering factors of two elementary models are analytically given, respectively, as Prigid ðqÞ ¼ N1
N X sin½ð2uÞsinðpn=NÞ
n¼1
ð2uÞsinðpn=NÞ
ð25Þ
and 2
u u Pflexible ðqÞ ¼ ð2=uÞexp D 2 4
ð26Þ
where u and D(x) denote the reduced scattering vector and the Dawson integral defined as uuqRG DðxÞ ¼
ðx
ð27Þ expðt2 Þdt
ð28Þ
0
The observed SAXS profiles from cyclic (1!2)-h-Dglucans exhibit a certain chain stiffness in comparison with the profiles calculated from the elementary models, where the conformational freedom is suppressed by linking endto-end. The Monte Carlo simulated scattering profiles reproduce the observed SAXS profiles reasonably well except for the deviation at the higher q region. The deviation at the higher q region may indicate that the effect of hydration should be taken into account, as no interference term due to the solvent–solute interaction is incorporated in the scattering profile calculation. However, the introduction of an apparent scattering unit smaller than 1.67 or 1.50 A˚ (for a carbon atom or an oxygen atom, respectively) reduces the deviation from the observed profile at u (u qRG) > 3 without any physical significance. A typical conformation is shown in Fig. 25 with space filling models, which reveal an irregular doughnut-like ring with the thickness of 10 A˚. The diameter of the CS21 ring annulus is about 4–5 A˚; that is, the cavity in a cyclic (1!2)h-D-glucan chain seems too small to embrace a relatively
Figure 24 Monte Carlo simulated and observed small-angle X-ray scattering profiles (the Kratky plots) of CS17 (a) and CS21 (b). The open circles denote the SAXS data, the solid lines the Monte Carlo simulated profile, the dotted lines the calculated profile for a rigid ring [Eq. (24)], and the broken lines the calculated profile for a Gaussian ring [Eq. (25)].
28
Kajiwara and Miyamoto
Figure 25 Space filling models of cyclic and linear (1!2)-h-D-glucan chains generated by the Monte Carlo method. CS21 (left) and LS21 (right) are seen from the top and the side. Hydrogen atoms are not included.
and 13.2 A˚ (LS21) from the SAXS data, or as 10.6 A˚ (LS 19) and 11.3 A˚ (LS21) from the Monte Carlo simulation. The discrepancy between the two sets of corresponding cross-sectional diameters evaluated independently accounts to some extent for the deviation of the scattering profiles at the larger q region. When the observed thickening is compensated by introducing larger radii for C and O atoms than the equivalent van der Waals radii, the consistency of the scattering profiles at the larger q region also improves. In Fig. 24, the scattering profile calculated from larger apparent scattering units (C and O atoms) shows a better fitting to the observed SAXS profile. The crosssectional diameter becomes approximately 12% larger by doubling the radius of the scattering units. Although the Monte Carlo simulation yields reasonably consistent results as a whole, more detail inspection reveals that the interaction with water (solvent) needs to be
considered to account for the interference effect at the higher q region. We have observed an opposite tendency of the interference effect at the higher q region in cyclic and linear (1!2)-h-D-glucan aqueous solutions. Although no physical significance is known at this stage, the apparent difference in the size of the scattering units may explain the mechanism of the physiological function found only in cyclic (1!2)-h-D-glucans.
IV. SUPRAMOLECULAR STRUCTURE OF POLYSACCHARIDES IN SOLUTION AND GEL Polysaccharides assume not a completely random a but quasi-ordered conformation in solution as shown in the preceding sections. This particular characteristic results in
Figure 26 Monte Carlo simulated and observed small-angle X-ray scattering profiles (the Kratky plots) of LS19 (a) and LS21 (b). The open circles denote the SAXS data, the solid lines the Monte Carlo simulated profiles with the radii of scatterers 1.67 A˚ (C) and 1.50 A˚ (O), the broken lines the Monte Carlo simulated profiles with the radii of scatterers 3.34 A˚ (C) and 3.00 A˚ (O).
Progress in Structural Characterization of Functional Polysaccharides
29
the formation of quasi-ordered domains in polysaccharide solutions. As a consequence, many polysaccharides form physical gel where the cross-linking domain is constituted of the quasi-ordered assembly of polysaccharide chains. The size of the quasi-ordered domain varies from a few nanometers to a few hundred nanometers, and the overall appearance of polysaccharide solutions and gels is determined by its size, structure, and the mode of its connection. This section deals with the structural characterization of quasi-ordered domains formed by oligo- and polysaccharides in solution.
A. Thermotropic Liquid Crystal of Cellulose Derivatives
Figure 27 Isotropization temperature Ti and melting temperature Tm as a function of side-chain length index for fully substituted cellulose derivatives; tri-O-alkyl cellulose (.) and cellulose trialkanoate (E).
Polysaccharide is hydrophilic and water-soluble in most cases as one of the most fundamental molecular characteristics. However, for example, cellulose is not water-soluble. The lack of solubility of cellulose in water is caused by numerous intra- and intermolecular hydrogen bonds. Cellulose is a linear polysaccharide consisting of anhydroglucose units linked by (1!4)-h-glucosidic bonds. The equatorial
Figure 28 Representative structures of poly- and oligosaccharide-based liquid crystals: (a) chiral nematic (cholesteric), (b) hexagonal columnar, (c) discotic hexagonal columnar, and (d) smectic A phase. Here (d) is supposed to be a structure for 1-Oalkyl-h-D-cellobiosides.
30
Figure 29 Transition temperature Ti (.) and Tm (o) for narrow fractions of fully decanoated cellulose.
configuration of the (1!4)-h-glucosidic bond predestines the stretched chain conformation of cellulose, which in turn promotes the intra- and intermolecular hydrogen bonds among their chains. The conformation of (1!4)-h-glucans is discussed in Sec. III.B in some detail. Another characteristic of cellulose is that almost all cellulose derivatives can form lyotropic liquid crystals because of the semirigidity of cellulose main chains. Chitin and its deacetylated derivative, chitosan, are also (1!4)-h-linked homopolysaccharides, and they can form lyotropic liquid crystals. Both cellulose and chitin can form fibers having good mechanical properties. Besides these, there occurs (1!4)-h-linked linear homopolysaccharide in nature. The properties of cellulose derivatives depend not only on the total degree of substitution (DS) and the molar substitution (MS) but also on (1) the distribution of substituents in the anhydroglucose (AHG) units (i.e., the relative DS and MS at three different types of hydroxyl groups), (2) the distribution of substituents along the cellulose chain, and (3) the distribution of DS and MS. The distribution within glucose unit arises because the three hydroxyl groups of the glucose residue generally differ in reactivity. This distribution can be estimated by 1 H and 13C NMR methods. On the other hand, the nonuniformity of the distribution along the chain is caused by heterogeneous reaction. In the case of copolymers, the control of compositional distribution is known to be very important to control their physical properties. The problem is equivalent to the control of the distribution of DS and MS values in the cellulose derivatives, although at present it is not easy to estimate their distributions. At all event, the substituent distribution control play a major role for the higher functionalization of cellulose [96–109]. An example is shown in the water solubility of the derivatives. Commercial methyl cellulose (MC) is watersoluble and shows a thermally reversible sol–gel transition in aqueous solution [103,110–112]. Commercial products are usually prepared by the so-called alkali cellulose process, which is based on a heterogeneous reaction. On the
Kajiwara and Miyamoto
other hand, MC samples prepared in a homogeneous phase with a nonaqueous solvent system shows no sol–gel transition. In general, the polymers possessing polar hydrophilic and nonpolar hydrophobic groups can dissolve in water, if water is a good solvent for the hydrophilic groups and any neighboring hydrophobic group is hydrated. However, when the temperature is increased, hydrogen bonds are weakened and hydration is reduced in the aqueous solution; that is, solvated hydrophobic groups lose their weakly bound water at higher temperatures. Consequently, they coalesce into a water-insoluble phase and the polymer precipitates at a certain temperature termed as a lower critical solution temperature (LCST) [112,113]. The cloud point is defined as the temperature at which turbidity is observed while heating a dilute solution slowly. Cellulose and chitosan are rich sources of lyotropic and thermotropic liquid crystals (LCs) [114,115]. As already described, both are linear, stereoregular polymers of D-glucose and D-glucosamine, respectively, linked by a (1!4)-h bond. This bonding together with the bulky
Figure 30
Four types of monomer units of xyloglucan.
Figure 31
Snapshots of xyloglucan monomer units with (1!4)-h-D-glucan spines on the right.
32
Kajiwara and Miyamoto
Figure 32 Small-angle X-ray scattering observed (black circles) and calculated (solid or dotted lines) from four types of tamarind seed xyloglucan monomer units. Since octasaccharide has two isomers (i.e., XXLG and XLXG), two dotted lines correspond to the respective scattering profiles from XXLG (above) and XLXG (below) and the solid line represents the calculated scattering profile as an average from the two isomers (30% XXLG and 70% XLXG in this instance).
Progress in Structural Characterization of Functional Polysaccharides
monomeric units forces the molecules to assume an essentially flat and extended conformation, affording these polymers and their oligomers mesogenic characters. Several studies have been reported on lyotropic and thermotropic cellulose derivatives. For a recent literature review on the lyotropic and thermotropic systems of these derivatives, the readers are referred to Ref. [116]. However, these studies are mostly concerned with HIPC-related derivatives. Those are chemically disordered polymers, the molecular structure–property relationships of which are difficult to establish. Here we describe the main features of thermotropic mesophases exhibited by fully substituted derivatives, which are chemically ordered polymers [115]. Fig. 27 demonstrates the phase behavior of two types of fully substituted cellulose derivatives, trialkyl celluloses and cellulose trialkanoates [117]. The abscissa scale N denotes the side chain length (i.e., the number of the C and O atoms forming the side chain skeleton). As N increases, the melting temperature Tm decreases drastically at first and seems to level off or slightly increases for N z 10, in all cases. Thus it is evident that the introduction of alkyl side chains effectively lowers the melting temperature of cellulose, but as the side chains become longer and the side chain fraction becomes larger, the melting behavior of the systems becomes more governed by that of the side chain components. Although the melting behaviors of the two mentioned systems are similar to each other, their mesomorphic properties are very different [118]. All cellulosic LCs, lyotropic or thermotropic, that were known in former times were cholesteric (or nematic). A cholesteric (chiral nematic) phase is characterized by the director field propagating in one direction, forming a helix of pitch P (Fig. 28a). The ether derivatives form a cholesteric phase in the vertically hatched region in Fig. 27, while the ester derivatives form quite a different phase in the horizontally hatched region. This phase is of a columnar hexagonal type [117]. The N dependence of the isotropization temperature Ti is also different for the ether and ester derivatives. The Ti of the ethers decreases with N rather monotonically, whereas that of the esters goes through a small maximum (Fig. 27). To be emphasized here is that though the difference in the chemical structures of these polymers is rather small, the observed differences in their mesophase properties may be surprisingly large. Fig. 29 shows the chain length dependence of transition temperatures Ti and Tm obtained for narrow fractions of fully decanoated cellulose and its oligomers [115,118,119]. This phase diagram consists of four regions—a crystalline solid region K, an isotropic liquid region I, and two mesomorphic regions D and C. The oligomeric phase D, which is relevant to homologs with DP < 5, is a discotic hexagonal columnar phase, as illustrated in Fig. 28c [120]. On the other hand, the polymeric phase C, relevant to homologs with DPw > 20 corresponds to the structure given in Fig. 28b [117]. Thus in the oligomeric phase, the molecular axis is perpendicular to the column axis, while in
33
the polymeric phase, it is parallel to the column axis. The transition from the perpendicular to the parallel orientation of the molecular axis is expected to occur at a DP of around 10, as Fig. 29 suggests, but it cannot be actually observed, as the transition temperature will be well below the melting temperature Tm. This behavior of the alkyl ester derivatives forms a remarkable contrast to that of the alkyl ether derivatives, which, as already described, form a chiral nematic phase when the chain lengths are sufficiently large. (Short alkyl ethers show no liquid crystallinity.) Acylated derivatives of chito-oligosaccharides also form a discotic hexagonal phase [121]. Owing to the hydrogen bonding interaction of the amide group, their phases have a higher stability than those of the cellocounterparts. The stability of the discotic hexagonal phase of the chito-compounds decreases with increasing DP of the main chain, and the derivative with a DP of 6 and a side chain carbon number of 14 is likely to form a discotic nematic phase [122].
B. Supramolecular Structure in Xyloglucan Gel Xyloglucan is a general term applied to nonstarch plant polysaccharides composed of a (1!4)-h-D-glucan with (1!6)-a-branched xylose, which is partially substituted by (1!2)-h-galacto-xylose [123]. Xyloglucan is normally contained in plant seed, and its flour has been traditionally used as a food additive in everyday life. Four types of monomer units are allocated to xyloglucan as designated as XXXG, XXLG, XLXG, and XLLG. Each unit is composed of a sequence of four (1!4)-h-D-glucans but differs in the number of galactose side chain (Fig. 30), so that the total number of sugar residues is 7 (in XXXG), 8 (in XXLG and XLXG), or 9 (in XLLG). Tamarind indica (TSP) and
Figure 33 Sol-gel transition temperature diagram of enzymatically degraded tamarind seed xyloglucan solution (1%).
34
Kajiwara and Miyamoto
Detarium senegalense are two common xyloglucans commercially available as a food additive, which have the same fundamental (1!4)-h-D-glucan spine with the different content of galactose with respect xylose and glucose. Four types of xyloglucan monomers were simulated by molecular dynamics, and the particle scattering function was calculated according to Eq. (12) from the atomic coordinates of the simulated xyloglucan monomer units [124]. The snapshots of simulated xyloglucan monomers
are seen in Fig. 31, together with respective (1!4)-h-Dglucan spines (without branches) shown on the right side. Here (1!4)-h-D-glucan spines are seen to assume rather flat zigzag conformation, and xylose and galacto-xylose branches to extend and fold upright on the (1!4)-h-Dglucan flat surface. In detail, nonasaccharide (xyloglucan monomer composed of nine sugar residues) exhibits a flatarched spin conformation, while octasaccharide (xyloglucan composed of eight sugar residues) and heptasaccharide
Figure 34 Molecular model for xyloglucan aggregate.
Progress in Structural Characterization of Functional Polysaccharides
35
Figure 35 Scattering profile from the model xyloglucan aggregates. The number of aggregated chains is indicated in the Figure.
36
Kajiwara and Miyamoto Table 6 Evaluated Parameters for the Tree-Like Model as a Function of Reaction Time Reaction time (min) 0 40 57 74 91 108
Weight fraction of ( f1)a
b (nm)
Single chain
14-Chain aggregate
0.45 0.5 1.0 1.04 1.06 1.07
6.0 11.0 13.5 13.7 14.0 14.0
1.0 0.49 0.24 0.13 0.07 0.05
0.0 0.51 0.76 0.87 0.93 0.95
(xyloglucan composed of seven sugar residues) assume a slightly twisted conformation. The loss of galactose side chains results in the increase of hydrophobicity, and seems to twist the backbone. A similar conformation of galactoxylose side chains is observed by Levy et al. [125] from the simulation by assuming a fixed flat (cellulose-like) or twisted (cellobiose-like) backbone conformation. Simulated scattering profiles are compared with the observed small-angle x-ray scattering profiles from tamarind seed xyloglucan monomer units in Fig. 32. The consistency of the simulated and observed results confirms the reality of the chain conformation visualized in Fig. 31. As gelation is prevented by the steric hindrance and hydrophilicity of (1!2)-h-D-galacto-xylose branches, the enzymatic degradation by h-galactosidase promotes gelation of xyloglucan aqueous solution [126]. At room temperature, tamarind seed xyloglucan aqueous solution forms gel at about 45% release of galactose residues, but this gel will melt at an elevated temperature. The resulted gel is opaque and has a unique property to have two melting points at lower and higher temperatures as shown in Fig. 33. The loss of (1!2)-h-galactose proceeds with a reaction time and more aggregation will take place to form cross-linking domains during the course of enzymatic degradation. Here the aggregation will take place laterally at the portion of xyloglucan chains lacking in terminal galactose. The aggregation is expected to form a quasiordered domain composed of laterally arranged xyloglucan chains. Because the conventional analysis of the observed small-angle x-ray scattering profiles indicate the formation of flat objects with 1.1-nm thickness upon gelation [50], the molecular model of a quasi-order domain was constructed by stacking cellulose-like (1!4)-h-D-glucan chains in parallel as shown in Fig. 34, and the scattering profile was calculated according to Eq. (12). Here the model consists of 14 xyloglucan chains each composed of 40 (1!4)-h-D-glucans with 30 (1!6)-a-xylose branches in the sequence of XXXG. (1!2)-h-galactose terminal groups are eliminated because the quasi-ordered domains are formed by the loss of these terminal groups. The scattering profile calculated from the model aggregate reveals distinguished peaks in the Kratky plots as the number of chains in the aggregate increases (Fig. 35). The small-angle x-ray scattering was observed from 1% tamarind seed xyloglucan aqueous solution during the
course of the enzymatic degradation. As the reaction time proceeds, the scattering profile at the medium q range becomes flat in the Kratky plots, while the profile at a higher q region remains almost invariant, exhibiting the characteristics of the rod-like scattering. The scattering curve at q ! 0 indicates to upturn after 57 min. This symptom is a typical behavior of the scattering from gelling systems [50]. Here gelation is assumed to take place according to the classic Flory-Stockmayer polyfunctional polycondensation scheme [127], and the scattering intensity from such a system is given as IðqÞ ¼ A2 ðaÞð1 þ a/Þ=½1 ðf 1Þa/
/ ¼ exp b2 q2 =6
ð29Þ
Here f denotes the functionality of the cross-linking domain (the number of branches from a domain), a the
Figure 36 Observed and calculated scattering profiles at various reaction times (indicated in the Figure). Symbols represent the observed small-angle x-ray scattering intensities and solid lines the scattering profiles calculated from Eq. (29) with A2( q) corresponding to the domain composed of 14 aligned xyloglucan chains.
Progress in Structural Characterization of Functional Polysaccharides
Figure 37
Chemical structure of lactose-carrying polystyrene.
conversion (the probability that an arbitrary chosen unit is reacted), b2 the mean square average of the distance between the neighboring scattering units, and A2( q) the scattering amplitude of each scattering unit [i.e., A2( q) = 1 in the case of a point]. The scattering amplitude A2( q) in the gelling system could be represented by the scattering factors of the domain composed of aggregated chains or a single chain of a certain length (Fig. 35). For simplicity, the gelling system of enzymatically degrading tamarind seed xyloglucan is assumed to consist of two phases of single chains (a dilute phase) and the domains of 14 parallel stacked chains (a condensed phase), and the observed scattering profiles are analyzed according to Eq. (29). The results are summarized in Table 6 and Fig. 36. The calculated scattering profiles are consistent with the observed profiles over the entire time course of enzymatically degrading reaction, although the condensed phase is not necessarily composed of 14 xyloglucan chains. Because no explicit number is known for the functionality f of a domain ( f should be equal to 24 if exactly 14 chains are
Figure 38 Small-angle x-ray scattering profile of VLA29, VLA92, and PVLA. The concentrations of each solution are the same (2 wt.%).
37
stacked in parallel to constitute a cross-linking domain), ( f 1)a should be regarded as a parameter to specify the average branching degree, where ( f 1)a = 1 indicates a gel point. The analysis involves three parameters—b, ( f 1)a, and the weight fraction of the domain composed of 14 aligned xyloglucan chains. The evaluated parameters are summarized in Table 6, and indicate that gelation takes place after 57 min of the reaction time in the present system. Table 1 also indicates that about 3/4 of chains are involved in the quasi-ordered domain at a gel point, and more single chains are incorporated into the quasi-ordered domains as further reaction takes place mainly on single chains after gelation. The thickness of the aggregated domain does not grow from 1.1 nm, and thus the domain seems to be composed of a single layer of stacked xyloglucan chains. At the end of reaction, most of the chains are incorporated
Figure 39 (a) Scattering profiles for three degrees of polymerization calculated from the molecular model of lactosecarrying polystyrene and (b) the fitting example for VLA92 where the symbols denote the observed SAXS intensities and a sold line represents the calculated profile for DP = 92.
38
Kajiwara and Miyamoto
in the thin domains, and the gel seems to be constituted of the cell-like network.
C. Glycoconjugate Synthetic Polymer Recent advances in the precise polymerization technique has resulted in synthesizing novel functional polymers mimicking biopolymers. Hybrids of synthetic polymers and biopolymers are of a particular interest, as the hybrid may enhance the characteristics of parent polymers. A series of glycoconjugate polystyrene derivatives have been synthesized with varying the types of pendant oligosaccharides [128]. The synthesized glycoconjugate polystyrene derivatives are amphiphilic with hydrophilic pendant oligosaccharides densely grafted on hydrophobic polystyrene main chain. Highly concentrated multiantennary glycol signals along hydrophobic main chain were in fact found to enhance the interaction with various types of carbohydrate-binding proteins, and the synthesized glycoconjugate polymers to function as a highly sensitive ligand [129]. For example, lactose-carrying polystyrene is suitable for the incubation of liver cells and the drug delivery systems [130]. Amphiphilic glycoconjugate polystyrene derivatives are water-soluble, as glycoconjugate polymers will form a single-molecule micelle in water to prevent precipitation. Three lactose-carrying polystyrene derivatives (the chemical structure is shown in Fig. 37) were prepared by radical homopolymerization or living radical polymerization of vinylbenzyl lactose amide [131]. The one prepared by radical homopolymerization (PVLA) has a high degree of polymerization with a broad molecular weight distribution, while the other two (VLA29 and VLA92) prepared by living radical polymerization have the degrees of polymerization of 29 and 92, respectively, with a narrow molecular weight distribution around 1.2. Small-angle x-ray scattering from the aqueous solutions of those samples (Fig. 38) reveals an identical profile at a high q region ( q > 0.1 A˚1) [132], indicating that the conformation of lactose-carrying polystyrene is almost the same regardless of the molecular weight and the SAXS profile difference at a low q region is due to the size of a whole molecule. The shape of both VLA92 and PVLA is approximately represented by a cylinder of the same cross-sectional radius as conformed from the cross-sectional Guinier plots of respective SAXS intensities, whereas VLA29 is not long enough to reveal the characteristics of a cylinder. The cylindrical shape of VLA 92 and PLLA could be accounted for by a polystyrene spiral backbone with protruding lactose side chains. Based on this conjecture, the molecular model of lactose-carrying polystyrene was constructed first by assuming an arbitrary sequence of trans–gauche (TG observed in the crystalline phase of isotactic polystyrene), trans–trans (TT observed in the crystalline phase of syndiotactic polystyrene), and trans– trans–gauche–gauche (TTGG observed in syndiotactic polystyrene) for a polystyrene spiral backbone, and secondly by linking lactose side chains as shown in Fig. 37 [132,133]. Then, the molecular model was simulated by the
Figure 40 Simulated molecular model of lactose-carrying polystyrene.
use of Cerius2 ver 3.5, and the particle scattering factor was calculated according to Eq. (12) for three lactose-carrying polystyrenes from the atomic coordinates of simulated molecular models. The results are shown in Fig. 39 including the fitting example for VLA92. The consistency of the calculated profile to the observed SAXS is satisfactory in all three cases, where VLA29 (a low degree of polymerization) can be represented by a shape of an ellipsoid rather than a cylinder. The simulated molecular model consists of a pseudohelical polystyrene backbone covered with lactose side chains (Fig. 40). The simulated molecular model confirms that the pseudohelical conformation of polystyrene backbone is retained even at DP = 29. Because polystyrene backbone is atactic, its conformation is random in principle but the backbone conformation is obliged to assume pseudohelical by the amphiphilic character of the backbone (hydrophobic) and side chains (hydrophilic). In this context, lactose-carrying polystyrene forms a singlemolecule cylindrical micelle.
ACKNOWLEDGMENTS The authors are indebted to Dr. Isao Wataoka, Dr. Hidekazu Yasunaga, and Dr. Mitsuru Mimura for their valuable comments during the preparation of the manuscript.
Progress in Structural Characterization of Functional Polysaccharides
REFERENCES 1. 2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21. 22.
23. 24. 25. 26. 27. 28. 29. 30. 31. 32.
Burchard, W.; Meuser, F., In Plant Polymeric Carbohydrates; Manners, D.L., Seibel, W., Eds.; The Royal Society of Chemistry: Cambridge, 1993. Glatter, O.; Kratky, O., Eds. Small Angle X-ray Scattering; Academic Press: London, 1982. Freeman, R. A Handbook of Nuclear Magnetic Resonance; Longman Scientific Technical: Harlow, U.K., 1988. French, A.D.; Brady, J.W., Eds. Computer Modeling of Carbohydrate Molecules, ACS Symposium Series 430; American Chemical Society: Washington, DC, 1990. Kacura´kova´, M.; Mathlouthi, M. Carbohydr. Res. 1996, 284, 145. Gress, M.E.; Jeffrey, G.A. Acta Crystallogr. 1977, B33, 2490. Quigley, G.J.; Sarko, A.; Marchessault, R.H. J. Am. Chem. Soc. 1970, 92, 5834. Takeda, H.; Yasuoka, N.; Kasai, N. Carbohydr. Res. 1977, 53, 137. Takeda, H.; Kaiya, T.; Yasuoka, N.; Kasai, N. Carbohydr. Res. 1978, 62, 27. Perez, S.; Vergelati, C.; Tran, V.H. Acta Crystallogr. 1985, B41, 262. Lamba, D.; Burden, C.; Mackie, W.; Sheidrick, B. Carbohydr. Res. 1986, 153, 205. Noguchi, K.; Okuyama, K.; Kitamura, S.; Takeo, K. Carbohydr. Res. 1992, 237, 33. Ikegami, M.; Noguchi, K.; Okuyama, K.; Kitamura, S.; Takeo, K.; Ohno, S. Carbohydr. Res. 1994, 253, 29. Perez, S.; Marchessault, R.H. Carbohydr. Res. 1978, 65, 114. Debye, P. Ann. Phys. (Leipz.) 1915, 28, 809. Guinier, A.; Foumet, G. Small-Angle Scattering of X-rays; Wiley: New York, 1955. Debye, P.; Bueche, A.M. J. Appl. Phys. 1949, 20, 518. Zierenberg, B.; Carpenter, D.K.; Hsieh, J.H. J. Polymer Sci., Polym. Symp. 1976, 54, 145. Kajiwara, K.; Burchard, W. Macromolecules 1984, 17, 2669. Flory, P.J. Statistical Mechanics of Chain Molecules; Interscience: New York, 1969. Kajiwara, K.; Hiragi, Y. In Applications of Synchrotron Radiation to Materials Analysis; Saisho, H., Goshi, Y., Eds.; Elsevier: Amsterdam, 1996. Kajiwara, K. The Method of Small-Angle X-ray Scattering and Its Application to the Structure Analysis of Oligosaccharides and Polysaccharides in Solution; Rome University: Rome, 1997. Shimode, M.; Urakawa, H.; Yamanaka, S.; Hoshino, H.; Harada, N.; Kajiwara, K. Sen’i Gakkaishi 1996, 52, 293. Hounsell, E.F. Progr. Nucl. Magn. Reson. Spectrosc. 1995, 27, 445. Farrar, T.C.; Becker, E.D. Pulse and Fourier Transform NMR: Introduction to Theory and Methods; Academic Press: New York, 1971. Bovey, F.A. High Resolution NMR of Macromolecules; Academic Press: New York, 1972. Bloembergen, N.; Purcell, E.M.; Pound, R.V. Phys. Rev. 1948, 73, 679. Bloembergen, N. Physica 1949, 15, 386. Carr, H.Y.; Purcell, B.M. Phys. Rev. 1954, 94, 630. Meiboom, S.; Gill, D. Rev. Sci. Instrum. 1958, 29, 688. Komoroski, R.A., Eds. High Resolution NMR Spectroscopy of Synthetic Polymers in Bulk; VCH, 1986. Andrew, B.R. In Progress in Nuclear Magnetic Resonance Spectroscopy; Emsley, J.W., Feeney, J., Sutcliffe, L.H., Eds.; Pergamon Press: Oxford, 1971; Vol. 8, Part 1, 1 p.
39
33. Andrew, E.R. Philos. Trans. R. Soc. Lond. 1981, A299, 505. 34. Hartmann, S.R.; Hahn, B.L. Phys. Rev. 1962, 128, 2042. 35. Pines, A.; Gibby, M.G.; Waugh, J.S. J. Chem. Phys. 1973, 59, 569. 36. Bax, A.; Davis, D.G.; Sarkar, S.K. J. Magn. Reson. 1985, 63, 230. 37. Bax, A.; Davis, D.G. J. Magn. Reson. 1985, 65, 355. 38. Macra, S.; Ernst, R.R. Mol. Phys. 1980, 41, 95. 39. Bax, A.; Davis, D.G. J. Magn. Reson. 1985, 63, 207. 40. Bothner-By, A.A.; Stephens, R.L.; Lee, J.-M.; Warren, C.D.; Jeanloz, R.W. J. Am. Chem. Soc. 1984, 106, 811. 41. Kollman, P. Chem. Rev. 1997, 93, 2395; van Gunsteren, W.F. Weiner, P.K., Wilkinson, A.J., Computer Simulation of Biomolecular Systems: Theoretical and Experimental Applications; Kluwer Academic: Dordrecht, 1997. 42. Koehler, S.E.H.; Saenger, W.; van Gunsteren, W.F. Eur. Biophys. J. 1988, 15, 197; J. Mol. Biol. 1987, 203, 241. 43. Woods, R.J.; Dwek, R.A.; Edge, C.J.; Fraser-Reid, B. J. Phys. Chem. 1995, 99, 3832; Woods, R.J. Reviews in Computational Chemistry; Lipkowitz, K.B. Boyd, D.B., Eds.; VCH: New York, 1995. 44. Maple, J.R.; Dinur, V.; Hagler, A.T. Proc. Natl. Acad. Sci., U. S. A. 1998, 85, 5350; Hwang, M.-J.; Ni, X.; Waldman, M.; Ewig, C.S.; Hagler, A.T. Biopolymers 1988, 45, 435. 45. Clark, A.H.; Ross-Murphy, S.B. Adv. Polym. Sci. 1987, 83, 57. 46. Wu, H.-C.; Sarko, A. Carbohydr. Res. 1978, 61, 7. 47. Imberty, A.; Perez, S. Biopolymers 1988, 27, 1205. 48. Rappenecker, G.; Zugenmaier, P. Carbohydr. Res. 1981, 89, 11. 49. Muller, J.J.; Gemet, C.; Schulz, W.; Muller, E.-C.; Vorweg, W.; Damaschum, G. Biopolymers 1995, 35, 271. 50. Kajiwara, K.; Kohjiya, S.; Shibayama, M.; Urakawa, H. Polymer Gels; Fundamentals and Medical Applications; DeRossi, D., Kajiwara, K., Osada, Y., Yamauchi, A., Eds.; Plenum: New York, 1991. 51. Leloup, V.M.; Colonna, P.; Ring, S.G.; Roberts, K.; Wells, B. Carbohydr. Polym. 1992, 18, 189. 52. Miles, M.J.; Morris, V.J.; Ring, S.G. Carbohydr. Polym. 1984, 4, 73. 53. Reuther, F.; Pleitz, G.; Damaschun, G.; Purschel, H.-V.; Krober, R.; Schijerbaum, F. Colloid Polym. Sci. 1983, 261, 271. 54. Shimada, J.; Kaneko, H.; Takaha, T.; Kitamura, S.; Kajiwara, K. J. Phys. Chem., B 2000, 104, 2136. 55. Goldsmith, E.; Sprang, S.; Fletterich, R. J. Mol. Biol. 1982, 156, 411. 56. Ikura, M.; Hikichi, K. Carbohydr. Res. 1987, 163, 1. 57. Hanessian, S.; Hod, H.; Tu, Y.; Boulanger, Y. Tetrahedron 1994, 50, 77. 58. Sarko, A.; Maggli, R. Macromolecules 1974, 7, 486. 59. Kolpak, F.J.; Blackwell, J. Macromolecules 1976, 9, 273. 60. Stipanovic, A.J.; Sarko, A. Macromolecules 1976, 9, 851. 61. Atalla, R.H.; VanderHart, D.L. Science 1984, 223, 283. 62. Horii, F.; Hirai, A.; Kitamaru, R. ACS Symp. Ser. 1984, 260, 29. 63. Cael, J.J.; Kwoh, D.L.W.; Bhattacharjee, S.S.; Patt, S.L. Macromolecules 1985, 18, 821. 64. Horii, F.; Hirai, A.; Kitamaru, R. Macromolecules 1987, 20, 2117. 65. Sugiyama, J.; Vuong, R.; Chanzy, H. Macromolecules 1991, 24, 4168. 66. Sugiyama, J. Cell. Commun. 1994, 1, 6. 67. Dudley, R.L.; Fyfe, C.A.; Stephenson, P.J.; Deslandes, Y.; Hamer, G.K.; Marchessault, R.H. J. Am. Chem. Soc. 1983, 105, 2469. 68. Raymond, S.; Chanzy, H. Cell. Commun. 1995, 2, 13.
40 69. Geissler, K.; Krauss, N.; Steiner, T.; Betzel, C.; Sandmann, V.; Saenger, W. Science 1994, 266, 1027. 70. Raymond, S.; Heyraud, A.; Tran Qui, D.; Kvick, A.; Chanzy, H. Macromolecules 1995, 28, 2096. 71. Raymond, S.; Henrissat, B.; Tran Qui, D.; Kvick, A.; Chanzy, H. Carbohydr. Res. 1995, 277, 209. 72. Tabata, K. Carbohydr. Res. 1981, 89, 121. 73. Gomaa, K.; Kraus, J.; Roßkoph, F.; Roper, H.; Franz, G.; Cane, I. Res. Clin. Oncol. 1992, 118, 136. 74. Yanaki, T.; Norisue, T. Polym. J. 1983, 15, 389. 75. Yanaki, T.; Norisue, T.; Fujita, H. Macromolecules 1980, 13, 1482. 76. Stokke, B.T.; Elgsæter, A.; Brant, D.A.; Kitamura, S. Macromolecules 1991, 24, 6349. 77. Kitamura, S.; Minami, T.; Nakamura, Y.; Isoda, H.; Takeo, K.; Kobayashi, H.; Mimura, M.; Urakawa, H.; Kajiwara, K.; Ohno, S. J. Mol. Struct. 1997, 395–396, 425. 78. Marchessault, R.H.; Deslandes, Y.; Ogawa, K.; Sundarajan, P.R. Can. J. Chem. 1977, 55, 300. 79. Bluhm, T.L.; Sarko, A. Can. J. Chem. 1977, 55, 293. 80. Deslandes, Y.; Marchessault, R.H.; Sarko, A. Macromolecules 1980, 13, 1466. 81. Bluhm, T.M.; Deslandes, Y.; Marchessault, R.H. Carbohydr. Res. 1982, 100, 114. 82. Sato, H.; Ohki, T.; Takasuka, N.; Sasaki, T. Carbohydr. Res. 1977, 58, 293. 83. Noguchi, K.; Kobayashi, E.; Okuyama, K.; Kitamura, S.; Takeo, K.; Ohno, S. Carbohydr. Res. 1994, 258, 35. 84. Harada, T. In Extracellular Microbial Polysaccharides; ACS Symposium Series; Sanford, P.A., Laskin, A., Eds.; Washington, DC: American Chemical Society, 1977; Vol. 45, 265 pp. 85. Saito, H. Annu. Rep. NMR Spectrosc. 1995, 31, 157. 86. Stipanovic, A.J.; Giammatteo, P.J. In Industrial Polysaccharides: Genetic Engineering, Structure Property Relations and Applications, Yalpani, M., Eds.; Elsevier: Amsterdam, 1987; 281 pp. 87. Saito, H.; Yoshioka, Y.; Yokoi, M.; Yamada, J. Biopolymers 1990, 29, 1689. 88. Fuchs, T.; Richtering, W.; Burchard, W. Macromol. Symp. 1995, 99, 227. 89. Guenet, J.-M. Thermoreversible Gelation of Polymers and Bioploymers; Academic Press: London, 1992. 90. Amemura, A.; Hisamatsu, M.; Mitani, H.; Harada, H. Carbohydr. Res. 1983, 114, 277. 91. Dell, A.; York, W.S.; McNeil, M.; Darvill, A.G.; Albersheim, P. Carbohydr. Res. 1983, 117, 185. 92. Miller, K.J.; Kennedy, E.P.; Rheinhold, V.N. Science 1994, 231, Breedveld, M.W.; Miller, K.J. Microbiol. Rev. 1986, 58, 145. 93. Abe, M.; Amemura, A.; Higashi, S. Plant Soil 1988, 64, Stanfield, S.W.; Jelpi, L.; O’Brochla, D.; Helinski, D.R.; Ditta, G.S. J. Bacteriol. 1982, 170, 3523. 94. Brant, D.A.; Mclntire, T.M. In Cyclic Polyssacharides in Large Ring Molecules; Semlyen, J.A., Ed.; Wiley: London, 1996. 95. Palleschi, A.; Crescenzi, V. Gazz. Chim. Ital. 1985, 115, York, W.S.; Thomsen, J.U.; Meyer, B. Carbohydr. Res. 1995, 248, 55; York, W.S. Carbohydr. Res. 1995, 278, 205. 96. Mimura, M.; Kitamura, S.; Gotoh, S.; Takeo, K.; Urakawa, H.; Kajiwara, K. Carbohydr. Res. 1996, 289, 25. 97. Burchard, W. Theory of Cyclic Macromolecules. In Cyclic Polymers; Semylen, J.A., Ed.; London: Elsevier Applied Science Pub., 1986. 98. Casassa, E.F. J. Polym. Sci. 1980, A3, Burchard, W.; Schmidt, M. Polymer 1965, 21, 745. 99. Lukanoff, B.; Philipp, B.; Schleicher, H. Cellul. Chem. Technol. 1979, 13, 417.
Kajiwara and Miyamoto 100. 101. 102. 103. 104. 105. 106. 107. 108. 109. 110. 111. 112. 113. 114. 115. 116. 117. 118. 119. 120. 121. 122. 123. 124. 125. 126. 127.
128. 129. 130. 131. 132. 133.
Miyamoto, T.; Sato, Y.; Shibata, T.; Tanahashi, M.; Inagaki, H. J. Polym. Sci., Polym. Chem. Ed. 1985, 23, 1373. Kamide, K.; Saito, M.; Akedo, T. Polymer Int. 1992, 27, 35. Aiba, S. Makromol. Chem. 1993, 194, 65. Takahashi, S.; Fujimoto, T.; Miyamoto, T.; Inagak, H. J. Polym. Sci., Polym. Chem. Ed. 1987, 25, 987. Daicel Chem. md., Ltd., Japanese Open Patent Sho 60– 42241, 1985, Taguchi, A.; Omiya, T.; Shimizu, K. Cell. Commun. Jpn. 1995, 2, 29. Sikkema, D.J.; Jannsen, H. Macromolecules 1989, 22, 364. Fukuda, T.; Sato, T.; Miyamoto, T. J. Soc. Fiber Sci. Technol. Jpn. 1992, 48, 320. Klemm, D.; Heinze, T.; Stein, A.; Liebert, T. Macromol. Symp. 1995, 99, 129. Miyamoto, T.; Long, M.; Donkai, N. Macromol. Symp. 1995, 99, 141. Philipp, B.; Wagenknecht, W.; Nehls, I.; Klemm, D.; Stein, A.; Heinze, T. Polym. News 1996, 21, 155. Kato, T.; Yokoyama, M.; Tukahashi, A. Colloid Polym. Sci. 1978, 256, 15. Donges, R. Br. Polym. J. 1990, 23, 315. Doelker, E. Adv. Polym. Sci. 1993, 107, 199. Mueller, K.F. Polymer 1992, 33, 3470. Guo, J.-X.; Gray, D.G. In Cellulosic Polymers, Blends and Composites; Gilbert, R.D., Ed.; Hanser Verlag: Munich, Chap. 2, 1994. Fukuda, T.; Takada, A.; Miyamoto, T. In Cellulosic Polymers, Blends and Composites; Gilbert, R.D., Ed.; Hanser Verlag: Munich, Chap. 3, 1994. Gilbert, R.D. Agricultural and Synthetic Polymers, ACS Symp. Ser.; American Chemical Society: Washington, DC, 1990; Vol. 433. Yamagishi, T.; Fukuda, T.; Miyamoto, T.; Yakoh, Y.; Takashina, Y.; Watanabe, J. J. Liq. Cryst. 1991, 10, 467. Fukuda, T.; Tsujii, Y.; Miyamoto, T. Macromol. Symp. 1995, 99, 257. Takada, A.; Fujii, K.; Watanabe, J.; Fukuda, T.; Miyamoto, T. Macromolecules 1994, 27, 1651. Itoh, T.; Takada, A.; Fukuda, T.; Miyamoto, T.; Yakoh, Y.; Watanabe, J. J. Liq. Cryst. 1991, 9, 211. Sugiura, M.; Minoda, M.; Fukuda, T.; Miyamoto, T.; Watanabe, J. J. Liq. Ciyst. 1992, 12, 603. Sugiura, M.; Minoda, M.; Watanabe, J.; Miyamoto, T. Polym. J. 1994, 26, 1236. York, W.S.; van Halbeek, H.; Darvill, A.G.; Albersheim, P. Carbohydr. Res. 1990, 200, 9. Yamanaka, S.; Mimura, M.; Urakawa, H.; Kajiwara, K.; Shirakawa, M. Sen’i Gakkaishi 1999, 55, 590. Levy, S.; York, W.S.; Stuike-Prill, R.; Meyer, B.; Staehelin, A.L. Plant J. 1991, 1, 195. Shirakawa, M.; Yamatoya, K.; Nishinari, K. Food Hydrocoll. 1998, 12, 25. Kajiwara, K.; Kohjiya, S.; Shibayama, M.; Urakawa, H. In Polymer Gels: Fundamentals and Biomedical Applications; DeRossi, D., Kajiwara, K., Osada, Y., Yamauchi, A., Eds.; Plenum: New York, 1991. See, for example Flory, P.J. Principles of Polymer Chemistry; Cornell UP: Ithaca, 1953. Kobayashi, K.; Sumitomo, H.; Ina, Y. Polym. J. 1985, 17, 567. Kobayashi, K.; Tsuchida, A.; Usui, T.; Akike, T. Macromolecules 1997, 30, 2016. Goto, M.; Yura, H.; Chang, C.-W.; Kobayashi, A.; Shinoda, T.; Maeda, A.; Kojima, S.; Kobayashi, K.; Akaike, T. J. Control. Release 1993, 28, 223. Ohno, K.; Tusjii, Y.; Miyamoto, T.; Fukuda, T.; Goto, T.; Kobayashi, K.; Akaike, T. Macromolecules 1998, 31, 1064. Wataoka, I.; Urakawa, H.; Kobayashi, K.; Ohno, K.; Fukuda, T.; Akaike, T.; Kajiwara, K. Polym. J. 1999, 31, 590.
2 Conformations, Structures, and Morphologies of Celluloses Serge Pe´rez and Karim Mazeau Centre de Recherches sur les Macromole´cules Ve´ge´tales, Grenoble, France
I. INTRODUCTION Photosynthetic organisms such as plants, algae, and some bacteria produce more than 100 million tons of organic matter each year from the fixation of carbon dioxide. Half of this biomass is made up of the biopolymer cellulose, which, as a result, is perhaps the most abundant molecule on the planet. This carbohydrate macromolecule is the principal structural element of the cell wall of the majority of plants. Cellulose is also a major component of wood as well as cotton and other textile fibers such as linen, hemp, and jute (ramie). For this reason, cellulose has always played an important role in the life of man, and its applications could even represent a landmark in the understanding of human evolution. Both fine lingerie and rough cottons have been recovered from the tombs of Egyptian pharaohs. Methods for the fabrication of cellulose substrates for writing and printing go back to the early Chinese dynasties. Cellulose and its derivatives are one of the principal materials of use for industrial exploitation ( paper, nitrocellulose, cellulose acetate, methyl cellulose, carboxymethyl cellulose, etc.) and they represent a considerable economic investment. This article provides a synthesis of the developments and conclusions of many of the multitude of studies that have been conducted on cellulose. Several reviews have been published on cellulose research [1–8] Necessarily, we have been selective and we have focussed on what we consider to be the most important events. Particular attention has been paid to the impact that the accumulation of structural knowledge of cellulose at its various organizational levels has had on the understanding of the biological and commercial function and properties of this remarkable biological material.
II. CELLULOSE AND ITS CELL WALL ENVIRONMENT Throughout their lifetime, the cells of living plants continue to divide with the production of certain cells, thus conferring the unusual property of being able to grow indefinitely while retaining the quality of young plants. These meristematic cells and those deriving from them grow and then differentiate into specialized cells for various functions, support, protection, flow of sap, etc. A collection of cells specialized for one function constitutes a tissue. Plant cell walls are distinguished from animal cells by the presence, around the plasmalemma, of a wall within which complex physicochemical and enzymatic phenomena progress. In the course of cell growth, the dimensions of the cell wall vary according to the type of macromolecule of which it is composed. The first wall deposited after cell division is called the ‘‘middle lamella’’ and is essentially composed of pectic material. The cell then lays down a wall composed of pecto-cellulosic material to supplant the middle lamella of the ‘‘primary’’ cell wall (Fig. 1). In fact, the primary cell wall is a glycoproteinaceous layer composed of pectin, cellulose, hemicellulose, and proteins. As the cell ages and differentiates, it secretes new materials, which form a mixture with the constituents of the primary cell wall, leading to the formation of a ‘‘secondary’’ cell wall. The nature of the constituents of the secondary cell wall depends on the cell type and tissue to which the cell belongs. In general, totally differentiated cells have stopped expanding and cannot divide further. Young plant cell walls represent a structure that is simultaneously rigid and dynamic. Indeed, rigidity is required to counterbalance the effect of turgor pressure on the plasmalemma. To allow cell extension to occur, the cell 41
42
Figure 1 Schematic representation of the plant cell walls along with the location of the main polysaccharides components. (From Ref. 143.)
wall structure must be deformable. This dual functionality of cell walls is achieved through the mixture of polysaccharides and proteins. Cellulose chains are formed into microfibrils, which constitute the basic framework of the cell conveying a great resistance to tensile forces [9]. The cellulose microfibrils represent about 20–30% of dry weight cell wall material occupying about 15% of cell wall volume. In cell walls that have differentiated and synthesized a secondary cell, the proportion of cellulose reaches 40–90% of the wall biomass [10]. The stages of cellulose biosynthesis involve transmembrane ‘‘rosettes’’ composed of hexamers of cellulose synthase [11]. The orientation and disposition of microfibrils in the wall are important because this more or less controls the capacity of the wall to deform and the direction in which the deformation can occur. In the final stages of cell wall differentiation, notably in the middle lamella and primary cell wall, other wall polymers (‘‘lignins’’) are incorporated into the spaces around the polysaccharide fibrillar elements to form lignin polysaccharides. Lignins arise from free radical polymerization of alcohols of para-hydroxy cinnamic acid and constitute between 10% and 30% of the dry weight of wood, placing them second to cellulose. They contribute to the mechanical strength of the plant cell wall and confer resistance to pathogens. Due to their hydrophobicity, they also confer resistance to water and control solute transport and water
Pe´rez and Mazeau
content. In the course of differentiation, cellulose microfibrils, associated with smaller molecules, hemicelluloses, and lignins, can provide a type of liquid crystalline matrix in which microfibrils can slide past one another, or else cause a disordered arrangement that resists further cell wall extension [9]. The hemicelluloses constituting a large number of different polysaccharide molecules actually form a matrix for the cellulose microfibrils involving molecular interactions such as hydrogen bonds and van der Waals forces. In addition to structural properties, hemicelluloses may also have other functions such as cell signalling, or as precursors of signalling molecules, or as reserve substances. Xyloglucans are major components of the hemicelluloses of higher plant dicotyledons and represent 20% of the dry weight primary cell wall material [5]. In monocotyledons, xyloglucan constitutes only 2% of dry material mass. In this case, xylans and h(1–3)-h(1–4)-glucans represent the major hemicellulose components with about 15–20% of dry weight cell wall mass. Xyloglucans, like the xylans, are closely associated with cellulose microfibrils through intermediary hydrogen bonds. Pectins constitute a major component of dicotyledon higher plants, about 35% of dry weight cell wall. In monocotyledons, their proportion is less and their type is different. Pectins represent a complex range of carbohydrate molecules whose backbone is composed chiefly of chains of a-D-(1–4) galacturonan interrupted by units of a-L-(1–2) rhamnose. The rhamnose-rich regions are frequently branched with side chains composed of neutral sugars of the arabinan/arabinogalactan type. These segments constitute the so-called ‘‘hairy’’ regions in contrast to unsubstituted galacturonan segments or ‘‘smooth’’ regions. In addition to structural and developmental functions, pectins are responsible for the ion exchange capacity of the cell wall and control of the ionic environment and pH of the cell interior. The plant cell wall contains a range of proteins, which are implicated in the organization and metabolism of the cell wall. The structural proteins can be gathered into five main families: extensins (rich in hydroxyproline), proteins rich in glycine (GRP), proteins rich in proline (PRP), lectins, and proteins associated with arabinogalactans (AGP). Cell wall enzymes may also be grouped into families according to function: (1) peroxidases that participate in the lignification processes of the cell wall; (2) transglycosidases that catalyze the breaking and making of glycosidic bonds in the cell wall; (3) a great number of hydrolases (glycosidases, glucanases, cellulases, polygalacturonases, etc.) and, just as important, esterases—a group of enzymes that constitute the machinery for the efficient degradation of the cell wall; (4) ‘‘expansins’’—proteins capable of rupturing the hydrogen bonds between cellulose microfibrils and xyloglucans [10]. A schematic representation of the primary cell wall of dicotyledons, showing the possible relationships between the principal components, is shown. Higher plant tissues such as trees, cotton, flax, sugar beet residues, ramie, cereal straw, etc. represent the main
Conformations, Structures, and Morphologies of Celluloses
43
sources of cellulose. Cellulose is also synthesized by bacteria such as Acetobacter. It is also found in a highly crystalline form in the cell walls of algae such as Valonia and Microdicyon. The animal kingdom also provides examples of several types of cellulose, of which the best studied is the membrane of marine animals belonging to the Ascite family commonly referred to as tunicates material [5]. Available evidence suggests that cellulose is formed at, or outside, the plasma membrane. Groups of rosette of particles or terminal complexes are seen in the plasma membrane. These groups of rosettes of particles can be seen to be associated with the ends of microfibrils (collection of cellulose chains) and are thought to be cellulose synthase complexes involved in the elongation of whole cellulose microfibrils. The catalytic subunit is a transmembrane protein with a transmembrane region. At the initiation of polymerization, two uridine 5c-diphosphate (UDP) glucose molecules are present in the substrate-binding pocket. As the chain elongates, glucose is added to the nonreducing end. The globular region of the protein is thought to be located in the cytoplasm, the UDP glucose being in the cytosol. A general model has been set to explain the molecular organization of the cellulose synthase molecules from the molecular level of organization to the rosette terminal complex level [12]. This complex is responsible for the synthesis of a microfribril that has 36 cellulose chains. Each of the six subunits of the rosette
must consist of six glucan synthase molecules. The hydrophobic regions coordinate the insertion of the hydrophilic domains on the cytoplasmic side of the plasma membrane, facilitating aggregation and association to form the rosette subunit particles. This particle is believed to synthesize glucan chain sheets [13], which have been shown to be the first products of the crystallization phase. Glucan chain sheets are then assemble to form the native cellulose (Fig. 2).
Figure 2 General model of the molecular organization of the cellulose synthase complex: the so-called ‘‘rosette terminal complex,’’ from which the crystalline cellulose I emerges. (From Ref. 144.)
III. CHEMICAL STRUCTURE OF THE CELLULOSE MACROMOLECULE Even though the early work of Braconnot [14] concerning the acid hydrolysis of the substance constituting plant cell walls goes back to the 19th century, it is with Payen [15] that the honor lies of establishing that the fibrous component of all plant cells has a unique chemical structure. It is also in the studies of Payen that the word cellulose was coined for the first time. However, it required another 50 years for the basic cellulose formula to be established by Willsta¨tter and Zechmeister [16] and for the volume of the crystalline mesh to be evaluated in 1921. The concept of cellulose as a macromolecule gave rise to a lively debate because the generally accepted idea was that the crystalline mesh corresponded exactly to the volume occupied by one molecule or a restricted number of molecules. It was due to the contribution of Staudinger [17] that the macromolecular nature of cellulose was finally recognized and accepted. Following this, Irvine and Hirst [18] and then Freudenberg and Braun [19] showed that 2,3,6-trimethyl glucose was the sole quantitative product resulting from methylation and hydrolysis of cellulose. This work showed that in cellulose, carbon atoms 2, 3, and 6 carried free hydroxyls available for reaction. Complementing these investigations were those in which, on one hand, the structure of glucose and cellobiose [20–22] was established and, on the other hand, those in which it was determined that cellulose was a homopolymer of h-(1–4)-linked Dglucopyranose. Crystallographical investigations of D-glucose and cellobiose [23] established unambiguously that the 4 D-glucose residues had the C1 chair conformation. All these investigations led to the establishment of the primary structure of cellulose as a linear homopolymer of glucose residues having the D configuration and connected by h-(1–4) glycosidic linkages (Fig. 3). The two chain ends are chemically different. One end has a D-glucopyranose unit in which the anomeric carbon atom is involved in a glycosidic linkage, whereas the other end has a D-glucopyranose unit in which the anomeric carbon atom is free. This cyclic hemiacetal function is in an equilibrium in which a small proportion is an aldehyde, which gives rise to reducing properties at this end of the chain so that the cellulose chain has a chemical polarity. Determination of the relative orientation of cellulose chains in the three-dimensional structure has been and remains one of the major problems in the study of cellulose.
Pe´rez and Mazeau
44
Figure 3
Schematic representation of the cellulose chain.
X-ray diffraction patterns obtained from fibrillar samples do not provide sufficient experimental information to resolve the crystallographical structure unambiguously. Indeed, a fiber is composed of an assembly of crystallites having a common axis but random orientation. To this source of disorder, that arising from the disorientation of the chains in the interior of the crystallite domains, along with their small dimensions, needs to be added. These various sources of disorder are the origin of the low number of reflections found in the fiber diagrams. On these diffractograms, the reflections are distributed in horizontal rows, the spacing of which corresponds to the fiber repeat when the polymer axis is parallel to the fiber axis. Thus, this periodicity is a geometrical parameter that can be determined unambiguously from a fiber diagram, and this usually corresponds to the c dimensions of the unit cell. Systematic absences of (0,0,1) reflections also provide information about the helical symmetry of the polymer chain. The possibility of unambiguous determination of the other unit cell parameters, as well as systematic absences in all the reciprocal space, depends on the ability to index the observed reflections, which, in turn, depends on the quality of the samples (Fig. 4). The conformation of the cellulose chain can be determined by means of molecular modelling, taking into account experimental data such as the helical parameters derived from the x-ray fiber diffraction diagrams. In the case of the cellulose chain, the conformational variations depend principally on the rotations around the glycosidic linkage. The first step involves construction of a map of the energies corresponding to the variations of the angles (U, W) that make up the glycosidic linkage. In the same way, it is possible to superimpose values of helical parameters on the iso-energy maps to permit the construction of a stable model (Fig. 5). The representation of the three-dimensional structure of the cellulose chain shows some key structural characteristics. As a consequence of the 4C1 chair conformation and the (1–4) glycosidic linkage of the h-D-glucopyranose residues, the structure is very much extended and corresponds to a twofold helix having a periodicity of 10.36 A˚ (Fig. 6). This conformation is situated in the low-energy zone in which van der Waals interaction and anomeric effect are optimized. An intramolecular hydrogen bond between O3 and the ring O5 of another residue provides additional stabilization (O5. . .O3: 2.75 A˚). This linkage is standard in cellulose chains with twofold symmetry, but is absent when other less stable conformations are derived under different
external environments. The exocyclic primary hydroxyl groups (O6) can adopt three low-energy conformations (gauche–gauche, gauche–trans, and trans–gauche) depending on a gauche stereoelectronic effect (Fig. 7). Although the trans–gauche conformation is rarely observed in the crystalline structures of oligosaccharides
Figure 4 Idealized fiber diffraction diagram from x-ray or Neutron scattering. An assembly of partially oriented blocks of microcrystallites (A) diffracts to produce large diffraction arcs (B). A perfectly oriented specimen (C) diffracts to give Bragg reflections on layer lines (D). (From Ref. 145.) The meridian reflection of the second layer lines indicates twofold helix symmetry. The periodicity along the linear macromolecule shows up a series of diffracting layer lines having a regular spacing, corresponding to the different orders of diffraction. The equator corresponds to the layer line 0, intersecting the non-diffracted central beam. The meridian is perpendicular to the equator and lies parallel to the fiber axis. The spacing along the meridian provides information about the periodicity of the macromolecule and its helical symmetry. The so-called helical parameters, n and h, are directly related to the symmetry of the macromolecular chain.
Conformations, Structures, and Morphologies of Celluloses
45
Figure 5 Potential energy surface computed for cellobiose as a function of U and W glycosidic torsion angles. The iso-energy contours are drawn by interpolation of 1 kcal mol1 with respect to the energy minimum. (From Ref. 146.)
Pe´rez and Mazeau
46
Glycosidic Torsion Angles and O3. . .O5V Distances for Cellobiose Fragments in Crystal Structures Compound
U (j)
W (j)
O3. . .O5V distance (A˚)
H-bond
O6V conformation
O6 conformation
Reference
h-cellobiose Me-h-cellotrioside (average of eight) Cellotetraose (average of six) Me-4O-Me cellobioside (monoclinic form) Me-4O-Me cellobioside (triclinic form) Me-h-cellobioside MeOH Cellulose II mercerized
76.3 94.4
132.3 146.6
2.77 2.864
Yes Yes
gt gt
gt gt
23 147
94.4 88.1
146.8 151.3
2.875 2.81
Yes Yes
gt gt
gt gg
80 148
90.0
159.2
2.76
Yes
gt
gg
148
91.1 96.8 93.3 95.4 95.1 98.8 88.7 98.0 99.0
160.7 143.5 150.8 147.7 150.6 141.9 147.1 138.0 140.0
2.76 2.79 2.75 2.78 2.76 2.77 2.70 2.47 2.92
Yes Yes Yes Yes Yes Yes Yes Yes Yes
gt gt gt gt gt tg tg tg tg
gg gt gt gt gt tg tg tg tg
149 83
Cellulose II regenerated Cellulose Ih Cellulose Ia
82 68 150
Figure 5 Continued.
[24], this conformation would yield a second hydrogen bond between chains (O2H. . .O6 = 2.87 A˚) that brings an extra stabilizing factor to the cellulose chain conformation. Nevertheless, it should be mentioned that cellulose can adopt other low-energy conformations, in particular at the interface of crystalline and amorphous zones where stacking constraint is less strong. Obviously, the possibilities for the formation of intrachain and interchain hydrogen bonds can give rise to various possibilities for the formation of stable three-dimensional structures. The possibilities are also reflected in differences of reactivity of the different functional groups, in particular in etherification reactions, because it has been shown that the hydroxyl groups O3 and O6 are much less reactive than O2. The degree of polymerization (DP) of native celluloses depends on the source and it is not well established. In fact, the combination of procedures required to isolate, purify, and solubilize cellulose generally causes scission of the chains. The values of DP obtained are therefore minimal and depend on the methods used [25,26]. Values of DP ranging from hundreds and several tens of thousands have been reported [26]. For the same reasons, the distribution of chain lengths of cellulose is not well established. Nonetheless, some authors suggest that the molecular mass distribution must be homogeneous for a cellulose of a given source [27].
IV. CRYSTALLINITY AND POLYMORPHISM OF CELLULOSE The free hydroxyl groups present in the cellulose macromolecules are likely to be involved in a number of intra-
molecular and intermolecular hydrogen bonds, which may give rise to various ordered crystalline arrangements. In the case of cellulose, these crystalline arrangements are usually imperfect to the extent that, in terms of crystal dimensions, even chain orientation and the purity of the crystalline form must be taken into consideration. The crystal density can be gauged from the crystallographical data, as can the importance of the amorphous components generally present. The density of the crystalline phase is 1.59 g cm3, but when determined for natural samples is on the order of 1.55 g cm3 [28], which corresponds to a value of about 70% for the crystalline component. The degree of crystallinity can also be estimated by infrared spectroscopy as a function of the relative intensity of certain bands [29]. Four principal allomorphs have been identified for cellulose: I, II, III, and IV [30]. Each of these forms can be identified by its characteristic x-ray diffraction pattern. Progress achieved in the characterization of cellulose ultrastructure has shown that within these four allomorphic families, subgroups exist. The relationships among the various allomorphs are shown schematically in Fig. 8. From Ref. [31]. The natural form of cellulose, called cellulose I or native cellulose, apparently is the most abundant form. Its three-dimensional structure is highly complex and not yet completely resolved as a result of the coexistence of two distinct crystalline forms, cellulose Ia and Ih. This was a major discovery and led to a revival of interest in the study of cellulose structure [32]. Cellulose I can be made to undergo an irreversible transition to a stable crystalline form, cellulose II, by two distinct processes: regeneration and mercerization. Cellulose II allomorph is known by the term ‘‘regenerated’’ cellulose. Regeneration involves either preparing a solution of cellulose in an appropriate solvent,
Conformations, Structures, and Morphologies of Celluloses
47
form cellulose IIII) or from cellulose II (which leads to the form IIIII). Cellulose III treated at high temperature in glycerol is transformed into cellulose IV. Here again, two types exist: cellulose IVI and IVII, respectively, obtained from cellulose IIII and IIIII. It is generally accepted that cellulose IVI is a disordered form of cellulose I. This could explain the reported occurrence of this form in the native state in some plants as determined by x-ray diffraction [33,34].
V. CRYSTALLINE STRUCTURES OF NATIVE CELLULOSES
Figure 6 Selected helical parameters n (number of residues per turn) and h (A˚) (projection of the residue on the helical axis) computed for a regular cellulose chain as a function of glycosidic torsion angles U and W. The iso-n and iso-h contours are superimposed on the potential energy surface for cellobiose. Arbitrarily, positive values of n and h designate a right-handed helix, and opposite signs will correspond to left-handed chirality. The screw sense of the helix changes to the opposite sign whenever the values n = 2 are interchanged. In practice, the regular parameters are readily derived from the observed fiber diffraction pattern (n = 2, h = 5.18 A˚). Values of the torsional angles consistent with the observed parameters are found at the intersection of the corresponding iso-h and iso-n contours. Discrimination between possible solutions is based on the magnitude of the potential energy.
or of an intermediate derivative followed by coagulation and recrystallization. This process is used to produce rayon fibers. Mercerization involves intracrystalline swelling of cellulose in concentrated aqueous NaOH followed by washing and recrystallization. This process is used to improve the properties of natural yarns and fabrics. The transition from cellulose I to cellulose II is not reversible, and this implies that cellulose II is a stable form compared with the metastable cellulose I (Fig. 9). Treatment with liquid ammonia or certain amines such as ethylene diamine (EDA) allows the preparation of cellulose III either from cellulose I (which leads to the
X-ray investigations of native cellulose samples were made 20 years ago following the early observations by optical microscopy, which suggested the existence of submicroscopical birefringent and oriented domains [35,36]. The analysis of x-ray diffraction patterns has played and continues to play a major role in structural studies of cellulose [28]. Prior to the discovery of the crystalline dimorphism of cellulose, most crystallographical studies concentrated on the determination of a basic unit cell. The controversy concerning the cellulose I unit cell dimensions and space group (believed to be unique) has lasted for many years in spite of the observations of various workers [37,38] who reported experimental data showing that diffraction intensities and spacings varied greatly depending on sample origin. For this reason, the literature is especially confusing on these points and is overloaded with conflicting experimental data and structural models.
Figure 7 4C1 chair conformation of a hexopyranose and Newman projections of the three staggered conformations about the C 5–C6 bond. In this figure, g and t are abbreviations of gauche (160j) and trans (180j), respectively, indicating qualitatively the value of a dihedral angle. The angle of the O6–C6–C5–O5 moiety is indicated by the first character and the angle of the O6–C6–C5–C4 moiety by the second character.
Pe´rez and Mazeau
48
Figure 8 Relationships among the different cellulose allomorphs.
A. Cellulose I From the x-ray diffraction pattern of cellulose from ramie, Meyer and Mark [39] proposed a monoclinic unit cell [a = 8.35 A˚, b = 7.0 A˚, and c = 10.3 A˚ (fiber axis), c = 84j] that served as a point of reference for a long time. The symmetry elements in the space group P21 are compatible with a twofold helicoidal symmetry for the cellulose chain and the authors proposed a structural model in which the chains were oriented in antiparallel fashion. Later, more elaborate studies, which took advantage of methods for resolving crystal structures and taking the packing energies into account, showed that the original proposal of Meyer and Misch represented an approximation. However, the principal modification to the original proposal concerned the chain orientation, which was concluded to be parallel in the crystalline lattice [40,41]. Studies on highly crystalline algal cellulose led to a reopening of the question of unit cell and space group proposed by Meyer and Misch. In particular, electron diffraction studies, made at low temperature on Valonia cellulose, produced results that were incompatible both with the unit cell dimensions and the space group symmetry proposed previously. The results, confirmed by independent studies, contradicted the twofold symmetry of the chain and suggested that Valonia cellulose had space group P1 and a triclinic unit cell [41,42].
arrangements with different dimensions [43,44]. It was 10 more years before the existence of two families of native cellulose was confirmed by the application of solid-state nuclear magnetic resonance (NMR) (13C CP-MAS) to a range of cellulose samples of different origins. From a detailed analysis of the carbon atom couplings observed
B. Celluloses IA and IB Away from the main controversy, other works suggested that celluloses from Valonia and bacterial sources had the same crystalline unit cell. Native celluloses of different origins might, in the same way, crystallize in different
Figure 9 Diffraction patterns of cellulose I and II after intracrystalline deuteration. (Courtesy of Dr. Y. Nishiyama.)
Conformations, Structures, and Morphologies of Celluloses
49
in the solid-state NMR spectrum, Atalla and VanderHart [32] and VanderHart and Atalla [45] established that native cellulose was a composite of two distinct crystalline phases named Ia and Ih (Fig. 10). The crystalline phases Ia and Ih can occur in variable proportions according to the source of the cellulose. The celluloses produced by primitive organisms (bacteria, algae, etc.) are enriched in the Ia phase, whereas the cellulose of higher plants (woody tissues, cotton, ramie, etc.) consists mainly of the Ih phase. Study of the cellulose of the outer membrane of marine animals showed that this is uniquely composed of the Ih phase. Hence, this cellulose may be considered to be the standard for the Ih phase [46]. Cellulose from Glaucocystis has been shown to consist of essentially cellulose Ia [47]. The discovery of the crystalline dimorphism of cellulose was the starting point for a number of research projects of which the aim was to evaluate the properties of each allomorph and procedures for their interconversion [48–52]. The observed reflections could be indexed to a monoclinical unit cell having space group P21 and dimensions a = 8.01 A˚, b = 8.17 A˚, c = 10.36 A˚, c = 97.3j. This unit cell is close to that proposed originally by Meyer and Misch from their work on cellulose from ramie, now known to be enriched in phase Ih. Phase Ia corresponds to a triclinic symmetry with space group P1 and dimensions a = 6.74 A˚, b = 5.93 A˚, c = 10.36 A˚, a = 117j, b = 113j, and c = 97.3j. The discovery of the crystalline dimorphism of cellulose and the existence of two families of native cellulose explained the number of inconsistencies that has characterized 50 years of the crystallographical study of cellulose. Thus, the eight-chain unit cell [53] can be explained as an artifact arising from the superimposition of the diffraction diagrams of phases Ia and Ih, which are both present in the Valonia cellulose. The occurrence of the dimorphism in native cellulose has been confirmed by systematic investigations of a wide range of samples by x-ray and neutron diffraction. The dimorphic concept has also allowed elucidation of several features of the spectra reported in infrared [54,55] and Raman spectroscopic studies [56]. In recent x-ray and electron diffraction studies, the space group and the chain packing of the Ia and Ih phases have been characterized [57,58]. Cellulose Ia has a triclinic unit cell containing one
chain, whereas cellulose Ih has a monoclinic unit cell containing two parallel chains, similar to the approximate unit cell proposed previously for cellulose I [40,41]. The ‘‘parallel-up’’ chain packing organization favored by Koyama et al. [59] has been confirmed by an electron microscopy study. These results have allowed a number of molecular descriptions for Ia and Ih to be produced by molecular modelling investigations [60–64]. There are also been a reexamination of the cellulose Ih structure determined from x-ray patterns of Valonia cellulose [65]. The experimental revision of the structure of cellulose I, in light of this dimorphism, awaited the development of new structural tools such as those provided by synchrotron, and neutron techniques. To achieve this, methods have been developed for deuteriation of the intracrystalline regions of native cellulose without affecting the overall structural integrity [66,67]. The neutron diffraction diagrams obtained in these studies are presented in Fig. 11 for cellulose I and II. These fiber diffraction diagrams are recorded at a resolution of 0.9 A˚, and several hundred independent diffraction spots can be measured by offering the promise of the establishment of unambiguous threedimensional structures. The deuterated fibers give highresolution neutron diffraction patterns with intensities that are substantially different from the intensities observed on neutron diffraction patterns obtained from hydrogenated fibers. The crystal structure and hydrogen-bonding system in cellulose Ih was elucidated by the combined use of synchrotron x-ray and neutron fiber diffraction [68]. Oriented fibrous samples were prepared by aligning cellulose microcrystals from tunicin, reconstituted into oriented films. These samples diffracted both synchrotron x-rays and neutron to better than 1 A˚ resolution, yielding more than 300 unique reflections and an unambiguous assignment of the monoclinic unit cell dimensions, (a = 7.784 A˚, b = 8.201 A˚, c = 10.380 A˚, c = 96.5j) in the space group P21. The x-ray data were used to determine the C and O atom positions. The positions of hydrogen atoms involved in hydrogen bonding were determined from Fourier difference analysis using neutron diffraction data collected from hydrogenated and deuterated samples. The chains are located on the 21 axes of the monoclinic cell. Therefore, they are not linked by any symmetry operation. The resulting structure consists of two parallel chains having slightly different conformations, both in terms of backbone and glucose conformations. All the hydroxymethyl groups adopt the trans–gauche conformation, which allows the formation of intrachain hydrogen bonding involving O2 and O6 groups interacting throughout multiple possibilities. In contrast, the O3. . .O5 intramolecular hydrogen bond is unambiguously well organized. Such a multiple hydrogen bonding scheme explains the complex OUC stretching bands observed in the infrared spectra of cellulose Ih [69]. The cellulose chains are organized in sheets packed in a ‘‘parallel-up’’ fashion. There are no intersheet OUH. . .O hydrogen bonds in cellulose Ih and, therefore, the cellulose sheets are held together by only hydrophobic interactions and weak CUH. . .O bonds.
Figure 10 Solid-state NMR spectrum of cellulose Ia and Ih. (From Ref. 32.)
50
Pe´rez and Mazeau
hydrogen atoms involved in hydrogen bonding was determined from a Fourier difference analysis using neutron diffraction data collected from hydrogenated and deuterated samples. The resulting structure is a one-chain triclinic unit cell of dimensions: a = 6.717 A˚, b = 5.962 A˚, c = 10.400 A˚, a = 118.08j, b = 114.80j, c = 80.37j, space group P1. The resulting structure consists of a parallel chain arrangement of the ‘‘parallel-up’’ type packed in very efficient way, the density being 1.61. Contiguous residues along the chain axis adopt a conformation remarkably close to a twofold screw, which is not required by the space group symmetry, all the hydroxymethyl groups being in a trans–gauche conformation. The occurrence of the intrachain hydrogen bond O3. . .O5 is found all over the structure with an alternation of two slightly different geometries. The hydrogen bonds associated with O2 and O6 are distributed between a number of partially occupied,
Figure 11 Description of the three-dimensional structure of cellulose Ih. (From Ref. 68.) (A) Neutron fiber diffraction pattern recorded on a hydrogenated sample (left) and on a deuterated sample (right). (B) Corey, Pauling, Koltun (CPK) representation and ball-and-stick representation of the layers of cellulose chains packed in a ‘‘parallel up’’ fashion in the monoclinic unit cell. (C) Details of the conformation of the two crystallographically independent chains, along with the hydrogen-bonding schemes. All the primary hydroxyl groups are in a trans-gauche orientation.
The occurrence of nonequivalent chains may provide an explanation for the fine details displayed by the 13C Cross Polarization-Magic Angle Spinning (CP-MAS) spectra of cellulose Ih [70]. The resonances assigned to the C1, C4, and C6 atoms exhibit distinct splitting. The different conformations of the glycosidic linkages and at the primary hydroxyl groups for the nonequivalent chains provide a structural explanation for these splittings. The crystal and molecular structures of the cellulose Ia allomorph have been established using synchrotron and neutron diffraction data recorded from oriented fibrous samples prepared by aligning cellulose microcrystals from the cell wall of fresh water alga Glaucocystis nostochinearum. The x-ray data recorded at 1 A˚ resolution were used to determine the C and O atom positions. The position of
Figure 12 Description of the three-dimensional structure of cellulose Ia. (From Ref. 150.) (A) Details of the conformation of two cellulose chains, made up of the alternation of slightly different conformations of the glycosidic linkages (U = 98j, W = 140j) and (U =98j, W = 138j), All the primary hydroxyl groups are in a trans–gauche orientation. (B) Projection of the relative orientation of the parallel chains of cellulose arranged in a parallel-up fashion in the triclinic unit cell. (C) CPK representation and ball-and-stick representation of the parallel layers of cellulose chains along the fiber axis.
Conformations, Structures, and Morphologies of Celluloses
51
but still well-defined, positions. As with cellulose Ih, these partially occupied positions can be described by two mutually exclusive hydrogen-bonding networks, and there is no hint of intersheet OUH. . .O hydrogen bonds (Fig. 12). Given the relationship between monoclinic and triclinic unit cells, as well as the Ia!Ih transformation by annealing in the solid state, it is likely that cellulose Ia also packs in a ‘‘parallel-up’’ fashion. The projections of the crystal structures of cellulose Ia and Ih down the chain axes are remarkably similar. As the projection perpendicular to the chain axis in the plane of the hydrogen-bonded sheets shows, the main difference is the relative displacement of the sheets in the chain direction. In both Ia and Ih, there is a relative shift of about c/4 in the ‘‘up’’ direction between neighboring sheets. The most likely route for solid-state conversion of cellulose Ia!Ib is the relative slippage of the cellulose chains past one another. Such a movement does not require the disruption of the hydrogen-bonded sheets (along the 010 planes for cellulose Ih, and 110 planes for cellulose Ia, but slippage by c/2 at the interface of the sheets). The exact location of the Ia and Ih phases along the crystalline cellulose microfibrils is another subject of interest. The respective components could be identified as alternating along the microfibril of the highly crystalline algal cellulose in the Microdiction cell wall [71] (Fig. 13). Modelling studies have established that the two crystalline arrangements correspond to the two low-energy
structures that could arise from parallel associations of cellulose chains. Within the framework of these studies, three-dimensional models have also been proposed, which allows comparison of the similarities and the differences that characterize the two allomorphs of native cellulose [63]. Several hypotheses have been proposed to account for the occurrence of two phases in native cellulose. In general, samples that are rich in Ia are biosynthesized by linear terminal complexes containing a number of cellulose synthases assembled in biological spinneret at the cell membranes. Those rich in Ih are organized in a rosette fashion [72]. However, a notable exception is tunicin, where linear terminal complexes produce almost pure Ih [91]. Obviously, the comparison between the morphology of Ih tunicin microfibrils with those of Ia-rich seaweed would be instructive. The former have a parallelogram shape, whereas the latter have a square shape. Therefore, despite their common linear geometry, the terminal complexes of tunicates and those of seaweeds produce microfibrils of different shapes and crystalline polymorphism. Obviously, other factors may play a key role in inducing cellulose crystalline structures.
Figure 13 The relationship between the unit cell of cellulose Ia and Ih.
VI. CELLULOSE II Early work on the solid-state structure of cellulose dates from 1929 [73] from which it was proposed that the unit cell had dimensions: a = 8.14 A˚, b = 14 A˚, c = 10.3 A˚, c = 62j and contained two cellulose chains. This proposal has caused little controversy in spite of the difficulty in indexing the x-ray diffraction reflections precisely. However, a larger unit cell (a = 15.92 A˚, b = 18.22 A˚, c = 18.22 A˚, c = 117j) was proposed on the basis of a neutron diffraction study [74], which called into question the previous assignment of the monoclinic space group P21. These variations could arise from the use of neutrons, which are sensitive to structural defects and disorder arising from the occurrence of various factors affecting the conformations of the positions of the hydrogen atoms in the hydroxyl groups. Besides, it could also be argued that the methods of preparation of this allomorph might account for some of the differences. There are indeed two main routes to cellulose II: mercerization, which involves treatment with alkali, and solubilization followed by regeneration (recrystallization). In spite of the similarities in unit cell dimensions, there are some differences that seem to be significant. For example, the values of the a dimension in a cellulose regenerated from ramie are 8.662 and 8.588 A˚ in the case of a cellulose obtained by mercerization. Similarly, the value of the angle g is always more significant for mercerized celluloses than for regenerated celluloses. It also seems likely that the degree of sample purity has a bearing on the quality of the crystalline domains and unit cell parameters, leading, as in the case of regeneration, to elevated rates of conversion [75]. There are few reports of the occurrence of the type II allomorph in native celluloses [76]. However, a structure corresponding to cellulose II has been proposed for a mutant strain of Acetobacter xylinum [77].
52
Several studies have been dedicated to structural determinations using a combined approach of x-ray diffraction data and modelling methods for minimizing the packing energies of cellulose chains in the unit cell [41,42,75,78]. In spite of some minor differences, the results agree sufficiently well to propose a model in which the cellulose chains have almost perfect twofold symmetry and are compatible with occurrence of two intermolecular hydrogen bonds between consecutive residues [OH3V. . .OU5 (2.70 A˚) and OH-2. . .O6V (2.70 A˚)]. Within the crystalline mesh, a network of hydrogen bonds ensures the formation of layers composed of cellulose chains. A notable feature of this three-dimensional arrangement is the antiparallel orientation of the cellulose chains. The similarities that exist between x-ray powder diffraction diagrams of cellulosic oligomers and that of cellulose II have excited the curiosity of crystallographers because it seemed likely that high-quality structural data from single crystals could be used to construct a model for the polymer. However, in spite of early success in crystallizing cellotetraose [79] and attempts at simulation, it was not until 1995 that the structure was resolved by two independent research groups [80,81]. Cellotetraose crystallizes in a triclinical unit cell (a = 8.023 A˚, b = 8.951 A˚, c = 22.445 A˚, a = 89.26j, b = 85.07j, c = 63.93j) having space group P1 containing two independent molecules. A major conclusion of these studies concerned the significant differences in the geometry of the two cellotetraose molecules, which were oriented in antiparallel fashion in the unit cell. The application of these new data to the resolution of cellulose II [80,81] has confirmed the conclusions of these studies with regard to the relative chain orientation, network of hydrogen bonds, chain conformation, and unambiguous assignment of the gauche–trans conformation of the primary hydroxyl groups, all in accord with spectroscopic data. Recent progress with methods of intracrystalline deuteration [66,67] has also made an important contribution to the elucidation of the cellulose II structure. Indeed, the combination of x-ray and neutron diffraction data has allowed the precise analysis of the complex network of intermolecular and intramolecular hydrogen bonding in cellulose II obtained by regeneration. This is the best model available for cellulose II [82]. In this model, the structure of cellulose II is based on a two-chain unit cell of dimensions a = 8.10 A˚, b = 9.04 A˚, c = 10.36 A˚, c = 117.1j. The chains are located on the 21 axes of the monoclinic cell and are antiparallel. The two chains have different backbone and glucose conformations. The glucoses of the central chain are strained and the chains are displaced relative to each other by about one fourth of the fiber repeat. The hydroxymethyl groups of the central chains are disordered and occupy both trans–gauche and gauche– trans positions. The precise location of hydrogen atoms provides the detailed description of the hydrogen-bonding system. A systematic three-center intrachain hydrogen bond is observed in both chains. This bond has a major component between O3 and O5, with O3 as a donor. A similar three-center hydrogen bond interaction occurs in
Pe´rez and Mazeau
the h-D-cellotetraose structure. The intermolecular hydrogen bonding differs substantially from that observed in hD-cellotetraose. One consequence of the difference is that O6 of the origin chain can donate a hydrogen bond to three possible acceptors, the major component being O6 of the center chain. These three acceptors already interact with one another through a three-center hydrogen bond. It is not clear as to what extent of disorder of the O6 group of the center chain is responsible for this intricate hydrogenbonding arrangement (Fig. 14). The use of synchrotron x-ray data collected from ramie fibers after ad hoc treatment in NaOH provided a revised crystal structure determination of mercerized cellulose II at 1 A˚ resolution [83]. The unit cell dimensions of the P21 monoclinic space group are a = 8.10 A˚, b = 9.04 A˚, c = 10.36 A˚, c = 117.1j. As with the regenerated
Figure 14 Description of the three-dimensional structure of cellulose II. (From Ref. 82.) Neutron diffraction patterns collected from two flax samples: once mercerized in NaOH/ H2O (left) and the other mercerized in NaOD/D2O (right). The fiber axis is vertical. Details of the conformation of the two crystallographically independent chains (‘‘origin’’: (U = 96.8j, W = 143.5j); ‘center chain (U = 93.3j, W = 150.8j). These chains are arranged in an antiparallel fashion in the unit cell. The hydroxymethyl group displays a gauche– trans orientation. A schematic representation of the hydrogen bonds in sheets containing only ‘‘origin chains’’ (C), only ‘‘center chains’’ (D), and ‘‘center’’ and ‘‘origin’’ chains. Intramolecular hydrogen bonds are O3UH. . .O5 in each molecule, with a minor component involving O6 as acceptor.
Conformations, Structures, and Morphologies of Celluloses
Figure 15 Projections of the structure of cellulose II along the fiber axis, along with the location of the chains in the monoclinic unit cell. CPK representation and ball-and-stick representation of the antiparallel layers of cellulose chains along the fiber axis.
cellulose, the chains are located on the 21 axes of the cell. This indicates that the different ways of preparing cellulose II result in similar crystal and molecular structures. The crystal structure consists of antiparallel chains with different conformations but with the hydroxymethyl groups of both chains near the gauche–trans orientation. There are, nevertheless, some significant differences between the conformations of the hydroxymethyl group of the center chain compared to that found in regenerated cellulose. This may be related to the difference observed in the amount of hydroxymethyl group disorder: 30% for regenerated cellulose and 10% for mercerized cellulose. Whether this disorder is confined to the surface of the crystallites or is pervasive is not known for the time being (Fig. 15).
VII. CELLULOSE III The crystalline forms of cellulose III (IIII and IIIII) are reversible and this suggests that, as with allomorphs I and II, the chain orientation is the same as in the starting material [84,85]. From unit cell dimensions a = 10.25 A˚, b = 7.78 A˚, c = 10.34 A˚, c = 122.4j, a structural model in which the chains did not have strict twofold symmetry was proposed. Several research investigations have focussed on the reversible transformations between cellulose I and III using techniques such as electron microscopy [86], solidstate NMR [50,51], x-ray diffraction [85], and molecular modelling [87]. From one study of the cellulose I–II transformation involving an intermediate cellulose I–EDA complex, it was concluded that a liquid crystalline phase was involved [87]. In the case of Valonia, the conversion from form I to II
53
was accompanied by an important decrystallization and fragmentation of the cellulose crystal. The reverse transition resulted in partial recrystallization, but this did not allow complete restoration of the damage done to the morphological surface. Characterization by electron diffraction revealed that the uniplanar–uniaxial orientation of the crystalline cellulose microfibrils was lost completely during the stage of swelling and washing necessary for the conversion into cellulose IIII. Washing with methanol resulted in the formation of irregularities into which were inserted crystalline domains of small dimensions. The final material that crystallized in the cellulose I form was obtained by treatment with hot water and characteristically displayed an increase in the accessible surface and consequently reactivity. Solid-state NMR studies have shown a significant decrease in the lateral crystallite dimensions during the transition of cellulose I–IIII. At the same time, the cellulose chains show conformational changes arising from the primary hydroxyl groups that change from a trans–gauche arrangement in cellulose I (65.7 ppm) to gauche–trans in the cellulose I–EDA (62.2 ppm) in the allomorph IIII. Thus, the regenerated cellulose I provides a spectrum that differs from that of the native form. Electron microscopy shows that cellulose I complexed with EDA is composed of nonuniform crystalline domains, whereas the III I allomorph is characterized by well-defined crystalline zones. The conformational changes observed for the primary hydroxyl groups are of interest because they provide possible markers for study of the various conformational transitions associated with cellulosic systems.
VIII. CELLULOSE IV Cellulose IVI and IVII allomorphs originate from cellulose I and II, respectively. The conversions are never totally complete, which explains the difficulties in the production of good-quality x-ray diffraction patterns [88]. However, unit cell dimensions have been obtained for the two allomorphs of which IVI has a = 8.03 A˚, b = 8.13 A˚, c = 10.34 A˚, which is close to those found for form IVII (a = 7.99 A˚, b = 8.10 A˚, c = 10.34 A˚) [89]. In both these cases, the poor quality of the diffraction patterns does not allow determination of the space group. The authors suggest space group P1 but this is not compatible with the proposed unit cell dimensions.
IX. ALKALI CELLULOSE Up to the present, research reports have tended to focus on the relative arrangement of cellulose chains in the cellulose I and II allomorphs. Whereas in native architectures the chains are parallel, regenerated or mercerized cellulose has antiparallel arrangements. Elucidation of the detailed events that take place during the transformation of cellulose I and II is of great interest, especially as the process of mercerization does not appear to require solubilization of the cellulose chains. It would seem therefore that the
Pe´rez and Mazeau
54
cellulose structure should be preserved. To understand the mechanisms that come into play, a great number of studies have been dedicated to the study of intermediate structures [90,91]. By means of characterization by x-ray diffraction, Okano and Sarko [92] put forward evidence for the occurrence of five different types of structure that could be classified as a function of the cellulose chain conformation. Soda celluloses of types I, III, and IV were characterized by a repeat of 10.3 A˚, whereas types IIA and IIB had a repeat of 15.0 A˚, corresponding to a helicoidal repeat of 3, a value not seen in previous studies. In addition, all the soda celluloses showed a reasonable degree of crystallinity and orientation. Hence, it seems difficult to reconcile a change of orientation with the mercerization process. These workers proposed that, because Na-cellulose I could not be converted back into cellulose I, the chains must be arranged in antiparallel fashion (i.e., as in cellulose II). Despite the failure to identify the mechanisms that come into play during the transformation from a parallel arrangement (cellulose I) to an antiparallel arrangement (cellulose II), these reports nevertheless have the merit of identifying the intermediate stage (Na-cellulose) from which the structural rearrangement could arise without chain solubilization. An extension of this research can be found in the studies of Hayashi et al. [91] in which nine types of Nacellulose, which could be formed from allomorphs I, II, III, and IV, were identified [93,94]. From these studies, it was concluded that the irreversibility probably depended more on conformational changes of the cellulose chain than chain rearrangements. This argument seems unconvincing because the energy differences between twofold and threefold helices are too small to account for the irreversibility observed for type I and II structures. Another tentative explanation was made from the occurrence of two types of microfibril in samples of Valonia: one of which had the chains oriented along the Oz crystal axis, the other having chains oriented in the opposite sense [95]. Most of the investigations dealing with mercerization of cellulose have focused on global measurements recorded on whole fibers (i.e., assembly of a large number of organized microfibrils). The structural and morphological changes accompanying mercerization of isolated cellulose microfibrils have been followed by transmission electron microscopy, x-ray, Fourier transform infrared spectroscopy (FTIR) and 13C CP-MAS NMR. The changes in morphology when going from cellulose I to cellulose II were spectacular as all the microfibrillar cellulose morphologies disappeared during the treatment. The outcome of this investigation is that is impossible for isolated cellulose microfibrils to become mercerized while keeping their initial morphology [96].
X. CRYSTALLINE MICROFIBRILS OF NATIVE CELLULOSE Much research has been devoted to experimental and theoretical studies of the crystalline component of native cellulose often in a context in which knowledge of the
molecular and crystallographical structure of native cellulose was lacking. It was during the 19th century that Hermans and Weidinger [28] developed a theory to deal with the birefringent materials in plant cells and starch grains. This theory led to the introduction of the concept of crystalline micelles having submicroscopical dimensions. This in turn led to the proposal that crystalline micelles were separate, well-defined entities that were stacked like bricks, whose length coincided with the axis of the constituent cellulose molecules. In order to take account of the amorphous content of cellulose, the idea of individual micelles evolved into the hypothesis of fringed micelles [97]. In this model, the micelles are considered to be ordered regions statistically distributed in a mass of chains that are more or less parallel. The interface between crystalline zones and amorphous zones is blurred and the micelle length need not necessarily correspond to the constituent chain length and a single chain may even pass through several micelles. The microfibrillar structure of cellulose has been established beyond doubt through the application of electron microscopy [98,99] and great variations in dimensions, depending on origin, have been reported [1,33,34]. The question of whether or not intermediate structural elements called elementary fibrils exist has been a topic of great controversy. However, the application of transmission electron microscopy [100,101] has established with certainty that the microfibril is the basic crystalline element of native cellulose [5,100–102]. It appears that the different levels of structural organization of cellulose are now well characterized.
A. Polarity of Cellulose Crystals The cellulose chain possesses a polarity that arises from the chemical difference of the two ends of the molecule and this confers particularly interesting properties to the crystalline architecture. In effect, two types of arrangement can be envisaged, depending on whether the reducing groups are all located at the same end of the chain assembly (parallel arrangement), or whether the reducing and nonreducing ends are arranged in alternating fashion within the assembly (antiparallel arrangement). The answer to this question has been the aim of numerous investigations but has equally given rise to a number of controversies. In their original model, Meyer and Misch [103] had proposed an antiparallel arrangement, which was supported by the observations of Colvin [104] on the production of bacterial cellulose in which the reducing ends of cellulose were stained with silver nitrate [105]. However, other attempts to identify reducing chain ends using conditions similar to those of Colvin were interpreted as supporting a parallel chain arrangement. It was from the use of exocellulases that final experimental proof of parallel arrangement [106– 108] in the family of native celluloses was finally obtained [109]. Recent investigations using complementary enzymatic and chemical staining of reducing ends have supported this model and, at the same time, produced precise descriptions of the orientation of the chains relative to the
Conformations, Structures, and Morphologies of Celluloses
55
crystal axes [59]. Hence, the crystalline microfibrils possess the same polarity as the chains of which they are composed. These conclusions are in agreement with the body of crystallographical and molecular modelling studies and reflect the constraints imposed by the biosynthetic requirements of native cellulose.
B. The Crystalline Morphology of Native Celluloses The availability of an accurate description of the crystalline structure of cellulose Ih, along with the predicted features of cellulose Ia, provides new insights into the crystalline morphology of native celluloses. These models can be used to generate different ordered atomic surfaces, and evaluate their occurrence along with their respective features. The schematic representation of the crystalline arrangements of cellulose Ia and Ih in relation with their respective unit cells is shown on Fig. 16. Irrespective of the fine structural differences, the same gross features are exhibited by the two polymorphs. This indicates that the same morphological features are expected to occur in the native celluloses. From such structural arrangements, well distinct types of crystalline surfaces can be identified. The type 1 surface represents the faces that run through the diagonal of the of the ab plane of the Ih monoclinical unit cell or through the a and b axis of the Ia triclinical unit cell. These surfaces are tortuous, displaying grooves extending parallel to the c axis. They are created by free spaces between the chains. Hydroxyl groups point outward, emphasizing the hydrophilic character
Figure 17 CPK representation of the main crystalline faces for cellulose I.
of these surfaces. The type 2 surface represents the faces that run through either the b axis of the Ih crystal or the first diagonal of the ab plane of the Ia crystals. The cellulosic chains exhibit C–H groups at the surface. This surface is flat and hydrophobic. The type 3 surface represents the faces that are parallel to the a axis of the Ih unit cell or to the second diagonal of the ab plane of the Ia crystals (Fig. 17).
C. Whiskers and Cellulose Microfibrils
Figure 16 Projection of the structure of cellulose Ia and Ih along the fiber axis. The triclinical and monoclinical unit cells are shown along with the main crystallographic directions, relevant for the crystalline morphologies.
Depending on their origin cellulose microfibrils have diameters from 20 to 200 A˚, whereas their length can achieve several tens of microns [5] (Fig. 18). These characteristics confer very interesting mechanical properties on microfibrils. Transmission electron diffraction methods have made a contribution to the quantification of the degree of crystallinity. Thus, using the technique of ‘‘image reconstruction’’ it was shown that, in the microfibril of Valonia, which has a diameter of about 200 A˚, there could be more than 1000 cellulose chains all aligned in parallel in an almost perfect crystalline array. Some imperfections arose from dislocations at the interface of microcrystalline domains along the microfibril length [100,110]. These imperfections were used to advantage by treatment with acid to produce monocrystals called ‘‘whiskers’’ having the same diameter as the starting microfibrils but much shorter length. These cellulose whiskers possess a mechanical modulus of about 130 GPa, which is close to calculated value for cellulose [111]. These characteristics (microscopical dimen-
Pe´rez and Mazeau
56
Figure 18 Range of microfibril size from different sources.
sions, form, and exceptional mechanical properties) made ‘‘whiskers’’ a choice ingredient in the manufacture of nanocomposite materials [112] (Fig. 19). Celluloses of different origin yield whiskers of diverse structural quality suitable for a range of applications. Hydrolysis of bleached tunicin cellulose (Halocynthia roretzi) with sulphuric acid yields monolithic microcrystals with a smooth appearance and lengths varying from hundreds of nanometers to several micrometers. The lateral dimensions of these monocrystals range from 50 A˚ to more than 200 A˚, which makes them 100 times superior with regard to form. The microcrystals obtained by hydrolysis of cotton linters are shorter than those from tunicin and reach lengths of 0.1 Am and widths from 10 to 50 A˚, and have a shape value of 20. At the other end of the spectrum, there are cellulose microfibrils from parenchyma that are quite different in appearance from those of cotton and tunimycin. These microfibrils are produced by a mechanical treatment, which, contrary to hydrolysis,
Figure 19
allows disruption of the microfibrils without affecting the original length. As a result, microfibrils several microns long and 20–30 A˚ wide are obtained (Fig. 20). Analysis of these different specimens by x-ray diffraction allows appreciation of the crystalline variation and the extent to which the amorphous components occur. The diffraction patterns of tunicin microcrystals are clearly of the allomorph I; they are detailed with welldefined rings. Those of cotton are less well defined and the rings are significantly more diffuse. In the case of parenchyma microfibrils, the resolution of the rings is less good and they begin to merge—a reflection of decreased lateral order and small size of the microfibril diameter. In contrast, longitudinal order is maintained along microfibrils of large dimensions. The amorphous phase increases as a result of decrease in microfibril diameter and the increase in the number of surface chains. The noncrystalline component essentially corresponds to the surface chains of which there will be more when the microfibrils are small. Fig. 21 is an idealized representation of the organization of cellulose chains, displaying morphology and dimensions typical of those of microfibrils of parenchyma. In such a case, the total number of cellulose chains would be 26; among them, 16 could be considered as surface chains. This finding has been corroborated by CP-MAS NMR applied to ultrathin cellulose microfibril extracted from sugar beet pulp [113]. It can be estimated that the surface chains in tunicin microfibrils constitute no more than 5% of the total number of tunicin chains, whereas surface chains can represent 70% of the total number in parenchyma microfibrils [5]. The result of increasing number of surface chains and decrease in whisker diameter can also be seen by
Electron micrograph of cellulose whiskers. (Courtesy of H. Chanty.)
Conformations, Structures, and Morphologies of Celluloses
57
Figure 20 Transmission electron micrographs of tunicin (A) microcrystals negatively stained with uranyl acetate. (B) Ultrathin section of microfibrils in bright field. Transmission electron micrographs of (C) cellulose microcrystals negatively stained with uranyl acetate. (D) Ultrathin section of a cotton fiber in bright field. Transmission electron micrographs of (E) parenchyma cellulose microfibrils negatively stained with uranyl acetate (F). (G) X-ray diffraction diagrams of cellulose microcrystals: (a) tunicin cellulose; (b) cotton; (c) parenchyma. (From Ref. 151.)
58
Figure 21 Molecular model of a microfibril of cellulose projected along the fibril axis compared to the typical morphologies observed for Tunicin and Valonia samples.
infrared spectroscopy by a broadening of the absorption bands with loss of resolution. It is believed that a peak at 1635 cm1 can be attributed to vibrations arising from water molecules absorbed in the noncrystalline regions of cellulose [114,115].
XI. SURFACE FEATURES OF CELLULOSES Many properties of native cellulose depend on the interactions that occur at the surface of the fibrils. As compared to bulk chains, surface chains are accessible and reactive. This is due to the dense packing of the chains within the crystal in which all the hydroxyl groups participate in crystalline cohesion through intramolecular and intermolecular hydrogen bonds. This structural understanding is supported by the many reported selective modifications of the cellulose fibrils, which occur only at the surface of the cellulose material. Surface chains play a fundamental role in the interaction processes (adsorption and adhesion) of the cellulose fibrils with other molecules. Such surface interactions play a key role in many scientific areas: biology (interaction with the plant cell wall polymers, adsorption of cellulolytic enzymes), industrial (paper and textile industries), and technological (compatibilization and adhesion a thermoplastic amorphous matrix on cellulose). Unfortunately, to date, very little information has been gathered on the organization, conformation, and dynamics of the surface chains. As a matter of fact, few experimental techniques can access the morphology of the material and surface
Pe´rez and Mazeau
interactions; furthermore, they are often delicate to implement and the obtained data are generally not easily exploitable. The organization of the surface chains has been initially studied by microstructural chemical analysis in which the reactivity of the exposed hydroxyl groups toward various chemical agents is tested [116–122]. Such experiments are analyzed under the assumption that only the exposed hydroxyls can react with an external chemical agent. Furthermore, hydroxyl group reactivity may be correlated with the degree of organization at the surface. An equivalent reactivity is expected for the different hydroxyls in the case of amorphous structure, in which the surface chains are not organized; this is a direct consequence of similar accessibilities. The specific reactivity of the O2H, O3H, and O6H hydroxyl groups toward various agents was measured [117] on cellulose samples differing in crystalline content. Such studies showed that hydroxyl group O2H is almost always available, in contrary to O3H hydroxyl, whose reactivity is strongly dependent on the crystalline index of the studied cellulose sample. The O3H is almost not susceptible toward chemical agents in highly crystalline Valonia or bacterial celluloses, in contrast to its measured reactivity in cotton cellulose for which the degree of organization is far less perfect. Hydroxyl group O6H shows an intermediate reactivity that also depends on the crystal index of cellulose. Those results are in good agreement with hydrogen-bonding network revealed from analysis of the neutron diffraction data of a deuterated tunicin sample [68]. Absence of reactivity of the O3H hydroxyl suggests that the strong O3H. . .O5 hydrogen bond observed in the crystalline structure persists at the surface of the cellulose materials, whereas larger reactivity of the O2H and O6H suggests that the hydrogen bonds involving those hydroxyls are at last partially disrupted at the surface. A larger conformational dynamics is therefore expected at the surface as compared to the one of the bulk. Organization of the surface chains of cellulose has been observed by atomic force microscopy (AFM) [123– 127]. The recorded AFM images obtained on Valonia samples highlighted that the surface chains are organized alike those of the bulk. A triclinic organization has been observed on Valonia ventricosa [123–125], whereas Valonia macrophysa displays a monoclinic organization of the observed surface chains [127]. High-resolution images obtained by Baker et al. showed the (100) face of the Ia triclinical allomorph. Periodicities of 10.4 and 5.2 A˚ were recorded, corresponding to cellobiose repeat along the fiber axis and interchain spacing (the distance between interreticular planes has been measured at 5.3 A˚), respectively. Triclinic organization was confirmed by the typical supermolecular arrangement of the chains, a diagonal shift close to 65j, corresponding to this allomorph, whereas discrimination between the (100) and (010) surfaces is based on the interreticular distance (Fig. 22). Finally, comparison between high-resolution images and reconstituted AFM image from crystallographic coordinates showed that the surface hydroxymethyl groups adopt a conformation that is different from the trans–
Conformations, Structures, and Morphologies of Celluloses
59
if all the different studies attempt to highlight the intrinsic characteristics of the surfaces (stability, hydrophilic and hydrophobic character, morphology, etc.), only few of them explicitly unravel the interactions between the surfaces of native cellulose and a guest molecule.
A. Congo Red
Figure 22 Atomic force microscopy of native cellulose. (From Ref. 124.)
gauche conformation of the buried groups. Molecular models of the surface of cellulose having either gauche– trans or gauche–gauche orientation of the hydroxymethyl group have a better agreement with the observed images. Such conformational differences disrupt the intramolecular (O2H. . .O6) hydrogen bond of the chains that are located at the surface of the cellulose material. It should be noted that all these AFM studies require an acid treatment of the samples to remove the disorganized chains initially present at the surface of the materials. Such chemical treatment allows an experimental observation of the surface in which the backbone conformation and the super molecular organization of the chains are close to that of the crystal. The majority of the AFM observations are supported by solid-state NMR [128,129]. In particular, NMR suggests that the orientation of the exposed primary (O6) group is in the trans–gauche and gauche–gauche orientations, in contrast with the trans–gauche orientation of the buried hydroxymethyl groups. NMR is a powerful tool to evidence the conformational disorder of the surface chains; it allows an estimation of the relative proportion of the different organization state of the fibrils of cellulose: crystalline bulk, organized surfaces, less-ordered surfaces, and amorphous domains [128]. It has been shown that the purification process, together with acid treatment, affects the ultrastructural organization of the chains [113]. The different experimental results show that the surface chains are partially disorganized; their conformational freedom is larger than the one of the bulk chains. The lesser amount of hydrogen bonds of the surface chains, as compared to the bulk ones, is consistent with a larger reactivity of those chains toward reactants and also for adsorbed species: water molecules, hemicelluloses, lignins, etc.
XII. INTERMOLECULAR INTERACTIONS In spite of the many structural investigations of cellulose, studies by molecular modelling remain surprisingly far from numerous. Furthermore, most of the efforts are devoted to the bulk: crystal packing prediction and estimation of mechanical properties. Studies concerning the surfaces of cellulose are extremely rare [130–135]. Finally,
Work performed by Woodcock et al. [130] aimed at energetical and geometrical characterization of the adsorption process of the aromatic organic dye, Congo red, on crystalline surfaces of cellulose with the help of molecular mechanics program, Assisted Model Building with Energy Refinement (AMBER). The considered surfaces are the (100) and (010) of the Ia phase, and the (1–10) and (110) of the Ih allomorph. Results suggest a preferential adsorption on the (010) of Ia and the (110) of Ih surfaces. Adsorption is mainly governed by the electrostatic contribution of the total energy between polar groups of the dye molecule and available hydroxyls and acetal oxygens of cellulose. Correlation between the calculated data and electronic microscopical experimental evidence [136,137] on adsorption of the cellulose-binding modules of cellulolytic enzymes on cellulose suggested that specific adsorption of cellulase might occur on the same surfaces of the modelled adsorption of Congo red. Such hypothesis has been recently revisited [138]; the cellulose-binding modules specifically adsorb on the (110) of the Ia phase of cellulose from Valonia. Nevertheless, preferential geometry of the complex has been reported from the arrangement that gives the lowest potential energy. Congo red is oriented parallel to the cellulose chains. In this study, the surface of the cellulose crystals is considered rigid; therefore, it does not consider possible structural disorganization and the enhanced mobility of the surface chains. Note also that no water molecules are included in the modelling protocol.
B. Benzophenone Surface chain mobility and structural disorganization have been considered in the work of Mazeau and Vergelati [135], which revealed the dependence of the cellulose surface characteristics on the adsorption behavior of benzophenone molecules. With the help of the Consistent Force Field (CVFF) force field, the geometrical and energetical characteristics of adsorption of benzophenone on crystalline (110), (1–10), and (200) of the Ih allomorph and an amorphous surface have been studied. Adsorption of benzophenone molecules has been modelled by using Monte Carlo and molecular dynamics protocols. Both (110) and (1–10) crystalline surfaces give similar results, whereas notable differences could be observed between these two surfaces and the (200). Among all the crystalline surfaces, adsorption occurs preferentially on the (200) surface. Interaction energies are of the same order of magnitude for all those crystalline surfaces. The principal energetical component that stabilizes the adsorption on the (200) surface is the van der Waals term, whereas the
Pe´rez and Mazeau
60
electrostatic contribution is important for the (110) and (1– 10) surfaces. Many adsorption sites have been identified for each surface. Adsorption of benzophenone has no preferential geometry on the (200) surface; on the contrary, the (110) and (1–10) surfaces for the geometry of adsorption appear strict. Finally, independently of the considered surface, a hydrogen bond is systematically observed between the carbonyl oxygen of benzophenone and a hydroxyl group of cellulose (Fig. 23). Benzophenone adsorbs flat on the (200) surface; the aromatic rings lie parallel to the surface of cellulose. In this preferential geometry, the aromatic rings are located above the apolar C–H groups of the surface chains, favoring hydrophobic stacking interactions. In spite of light structural differences between the (110) and (1–10) surfaces, the adsorption process of benzophenone is the same for these two surfaces. The authors also studied the formation of a benzophenone monolayer on (1–10), (200), and amorphous surfaces. On the crystalline surfaces, the adsorption sites are qualitatively identical and are periodically repeated on the surface. On the contrary, the amorphous surface of cellulose shows sites that are topologically extremely favorable to the benzophenone adsorption for which the interaction energy is large. Once those remarkable sites are fulfilled, benzophenone molecules adsorb on sites that are energetically comparable to the crystalline ones. Finally, stability and time evolution of the adsorbed monolayer of benzophenone at the interface with liquid water were tested by recording molecular dynamics trajectories. Differences in the density profiles between the initial structures and the structures obtained after 1 nsec of molecular dynamics experiment show a light reorganization of the crystalline surfaces and benzophenone molecules remain located at the surface within the time scale of
the experiment. On the contrary, for the amorphous surface, benzophenone molecules significantly penetrate within the cellulose material.
C. Water Heiner and Teleman [132] and Heiner et al. [133] performed molecular dynamics simulations on an interface between crystalline cellulose and water, by using the Gronengen Molecular Simulation System (GROMOS) force field. The considered surfaces are the (010) and (100) of the triclinical phase and the (100) and (1–10) of the monoclinical one. Each modelled system is composed of six layers of cellulose chains; each layer is constituted by six chains of six glucose residues. This cellulose material is solvated by explicit water molecules. Analysis of the geometrical and conformational parameters shows that only the topmost cellulose layer is affected by the presence of water molecules. This result is in good agreement with solid-state NMR data, which show that the surface effective component of the spectra corresponds to a single layer [128]. Dynamics and conformation of the surface chains differ from the bulk chains. In particular, hydroxymethyl group conformation possesses a marked rotational freedom; gauche–trans is the preferred orientation, in opposition with the trans–gauche conformation of the hydroxymethyl group of the bulk chains. The decrease of hydrogen bonds at the surface of the cellulose is compensated by hydrogen bonds between cellulose and water. The O3H–O5 intramolecular hydrogen bond persists at the surface, in agreement with the conclusions derived from microstructural chemical analysis (Fig. 24). Hydration of the surfaces has been estimated from density profiles of the water molecules, which clearly
Figure 23 Molecular representation of the adsorption of benzoophenone on crystalline cellulose. (From Ref. 135.)
Conformations, Structures, and Morphologies of Celluloses
61
same approach, but for an argon atom, which is a model of lipophilic molecules. Data showed that the two surfaces are equivalent, nonhydrophilic, and mainly lipophilic. Water molecules are not attracted by the surface.
D. Lignin
Figure 24 Hydration of cellulose as seen from molecular dynamics simulations. (From Ref. 132.)
indicate water structuring close to the surfaces. Because of the interactions between cellulose and water, the dynamics of the water molecules decreases by a factor of 2–3 close to the surface. It is also found that monoclinic (110) and triclinic (010) surfaces behave similarly just as the monoclinic (1–10) and triclinic (100) ones. These two last surfaces have a larger hydrophilic character than the two others. Hydrophilic character of the surface has been shown to be dependent on hydroxyl group distribution on the surface together with their ability to maximize hydrogen bonds. Hydrophilic and lipophilic character of the cellulose surfaces has been independently estimated by Biermann et al. [134], using molecular dynamics calculations. The modelled systems consist of an interface of cellulose, exposing their monoclinic (110) and (1–10) surfaces, and water. Hydrophilic character was estimated from local values of the chemical potential of water close to the surface with respect to its value far from the surface, in the bulk. Lipophilic character was estimated by using the
The hypothesis of association between lignin building blocs on the surface of the cellulosic matrix was tested by modelling. Houtman and Atalla [131] studied the dynamical behavior of model compounds that are lignin precursors (monolignols and trilignols) in the presence of a hydrated surface of crystalline Ih cellulose. Although initially located in the aqueous phase, at about 13 A˚ of the cellulose surface, modelling evidenced a rapid adsorption of the monolignol on the cellulose surface. Results showed that the driving force responsible for adsorption is mainly of electrostatic nature. Interactions between the monolignol and the cellulose chains are strong enough to influence the dynamics of the adsorbate close to the surface. Mobility of the monolignol is considerably decreased when the molecule reaches the surface. As a consequence of this limited mobility, the preferred adsorption geometry of the lignols is parallel to the cellulose fiber axis and the aromatic moieties of lignols are parallel to the cellulose surface; thus, hydrophobic interactions are maximized through stacking-type interactions. Also, a fast adsorption of the trilignol model was observed. It adsorbs flat on the surface and two of the three aromatic rings are oriented parallel to the surface. On the basis of those results, authors confirm that the cellulose fibers and, more generally, the polysaccharide matrix, can influence monolignol polymerization and ultrastructural organization of lignin in the plant cell walls. Such adsorption leads to a reorganization of the lignin structural units before polymerization, which could influence the primary structure of the lignin polymer through selected distribution of the monomer units and also could influence the conformation of the lignin polymer. Work performed by Jurasek [139] also suggests that cellulose might influence the structure of the lignin polymer. The growing of a bidimensional model of the secondary cell wall is faster in the direction parallel to the fiber axis than in the perpendicular direction. Spatial
Figure 25 Schematic representation of wood fiber structure. P, primary cell wall; S2, middle secondary cell wall; S1, outer secondary wall; S3, inner (tertiary) cell wall.
62
Pe´rez and Mazeau
Conformations, Structures, and Morphologies of Celluloses
Figure 27
63
Structural levels of organization of cellulose in the plant cell wall.
Figure 26 Microfibril organization in wood. (From Ref. 142.) (A) Wood cells in cross section were scanned by a microbeam smaller than the thickness of a single cell wall. The tilt angle of the cellulose fibrils with respect to the beam corresponds to the microfibril angle l. (B) A perfect alignment of all crystallographic axes of cellulose would yield sharp diffraction spots corresponding to the (0 2 0), (1 2 0), (1 1 0) reflections in the plane perpendicular to the fibril axis in the reciprocal space. A random orientation of the fibrils around their longitudinal axis would result in a smearing of the reflections to rings. (C) Principle for the measurement of local fibril orientations. (i) Cellulose fibril tilted by an angle l with respect to the incoming X-ray beam: a / denotes the orientation of the fibril in the plane perpendicular to the beam. (ii) In reciprocal space, the smearing of the reflections [(0 2 0), large ring; (1 1 0) + (1 1 0), small ring] is caused by random orientation of the parallel cellulose fibrils around their longitudinal axis. A and B are the points of intersection between the Ewald sphere and the Debye–Scherrer rings. (iii) Scattering pattern as it would appear on the area detector in the plane perpendicular to the beam. The scattering pattern is asymmetrical. The orientation af of the cellulose fibrils (indicated by an arrow) can be extracted directly form the peak position. (D) Mesh scan over a complete wood cell in cross section with part of neighboring cells; pixel size: 2 2 mm. Dark region correspond to lumina; bright region showing a scattering signal corresponding to cell walls. (b) Two typical diffraction patterns (with greater magnification) showing the local orientation of the cellulose fibrils af, denoted by arrows. (E) Map of local cellulose fibril orientations. Following the arrows readily yields the trace of the fibrils around the cell. Longer arrows denote a more pronounced asymmetry of the diffraction patterns corresponding to smaller local fibrils angles; shorter arrows denote larger fibril angles. (F) Translation of the arrow map into a three-dimensional model; the cellulose fibrils trace a helix around the cell.
Pe´rez and Mazeau
64
constraints due to the presence of the cellulosic matrix impose a certain degree of regularity in the final structure of lignin. Molecular mechanics calculations performed by Faulon and Hatcher [140] suggest that the helical conformations of lignin oligomers are energetically preferred than random coils. This is in agreement with experimental observation of lignin by scanning tunneling microscopy; images show an ordered structure [141].
XIII. MICROFIBRIL ORGANIZATION In nature, cellulose is most commonly found as part of an architectural complex whose ultrastructural organization depends on the organism under consideration. In a material such as wood, which is rich in cellulose, the cell walls are composed of cohesive, interlaced crystalline microfibrils that are themselves composed of cellulose (Fig. 25). The cellulosic fibers are 1–2 nm long and about 35 A˚ wide and the microfibrils are composed of 30–40 cellulose chains. Application of new approaches using synchrotron radiation has made a momentous contribution to the characterization of their structural organization [142] (Fig. 26). X-ray diffraction diagrams have been recorded, using wavelengths of 0.78 A˚, on wood sections about 10 Am thick oriented perpendicularly to the incident beam. The specimen under investigation (52 42 Am) was scanned in increments of 2 Am, resulting in a collection of 26 21 diffraction patterns, which provided a distribution map of the orientation of the axes of the cellulose microfibrils. In effect, each diffraction diagram is characterized by strong intensities, which were attributed to (0, 2, 0), (1, 1, 0) and (1, 1, 0), so that the orientation of the microfibril along the direction of propagation could be deduced. The outcome of such an exploration is shown schematically, in which the dark areas where no diffraction is recorded are considered to arise from the lumen. Analysis of each diagram for its part allows determination of the local orientation of the microfibril axis. Integration of the individual observations gives an image of the degree of disorientation. The big arrows indicate a marked local asymmetry in the microfibrils and thus that amplitude is of less importance than the local orientation of the microfibril. Translated into three dimensions, these results lead to an ultrastructural model in which it is established that the orientation of the cellulose fibrils is aligned with the cell axis in a superhelicoidal fashion.
where knowledge is incomplete. The structure and dynamics of chains at the crystallite surface are also not well established and the study of outer chains is likely to become an important topic for future research using techniques such as solid-state NMR, near-filled microscopy, molecular modelling, mechanical spectroscopy, etc. The nature of the topological changes that accompany the transitions between the different cellulose polymorphs also remains to be more firmly established. Without doubt, better knowledge of the different structural levels in which cellulose participates will permit better use of this unique and metastable molecular assembly, which is produced by biosynthesis. The numerous classical applications of cellulose, depending on factors such as the macromolecular nature of the chain or as a component of wood, will soon be complemented by applications involving ‘‘whiskers’’. Thus, the industrial applications for cellulose will continue to grow. For this to be put into operation, understanding of the modification of the heterogeneous phase by chemical and enzymatic means will be needed to confer new properties on the macromolecular chain assemblies of cellulose.
ACKNOWLEDGMENTS The authors express their gratitudes to Drs. H. Chanzy, Y. Nishiyama and J. F. Sassi.
REFERENCES 1. 2. 3. 4.
5.
6. 7.
XIV. CONCLUSIONS The data gathered together in this article have followed the development of knowledge of the different structural levels of cellulose. These concern: chain conformation, chain polarity, chain association, crystal polarity, microfibril structure, and organization. All these structural levels are presented schematically, including their relationship to the plant cell wall (Fig. 27). Many structural features have been firmly established, and there remains relatively few areas
8. 9. 10. 11. 12.
Preston, R.D. X-ray analysis and the structure of the components of plant cell walls. Phys. Rep. 1975, 21, 183–226. Preston, R.D. Natural cellulose. In Cellulose: Structure, Modification and Hydrolysis; Young, R.A., Rowell, R.M., Eds.; John Wiley and Sons: New York, 1986, 3–27. Marchessault, R.H.; Sundararajan, P.R. In Cellulose. In The Polysaccharides; New York: Academic Press, 1983, 11–95. Sarko, A. Cellulose—how much do we know about its structure? In Wood and Cellulosic Industrial Utilization, Biotechnology, Structures and Properties; Kennedy, J.F., Ed.; Ellis Horwood: Chichester, UK, 1987, 55–70. Chanzy, H. In Cellulose Sources and Exploitation, Aspects of Cellulose Structure. Kennedy, J.F., Phillips, G.O., Williams, P.A. Eds.; Ellis Horwood Ltd.: New York, 1990, 3–12. Okamura, K. Structure of cellulose. In Wood and Cellulosic Chemistry; Hon, D.N.S.-S., Shiraishi, N., Eds.; Marcel Dekker: New York, 1991, 80–111. O’Sullivan, A. Cellulose: the structure slowly unravels. Cellulose 1997, 4, 173–207. French, A.D. Structure and biosynthesis of cellulose: I. Structure and biosynthesis of cellulose. Discov. Plant Biol. 2000, 3, 163–197. Jarvis, M.C. Structure and properties of pectin gels in plant cell walls. Plant Cell Environ. 1984, 7, 153–164. MacQueen-Mason, S.J.; Durachko, D.M.; Cosgrove, D.J. Two endogenous proteins that induce cell wall extension in plants. Plant Cell 1992, 4, 1425–1433. Taiz, L.; Zeiger, E. Plant Physiology. The Benjammin/ Cumming Publishing Company, 1991. Malcom Brown, R.; Saxena, I.M., Jr. Cellulose biosyn-
Conformations, Structures, and Morphologies of Celluloses
65
thesis: a model for understanding the assembly of biopolymers. Plant Physiol. Biochem. 2000, 38, 57–67. Cousins, S.K.; Brown, R.M., Jr. Cellulose I microfibril assembly: computational molecular mechanics energy analysis favour bonding by van der Waals forces as the initial step in crystallization. Polymer 1995, 36, 3885–3888. Braconnot, H. Sur la conversion du corps ligneux en gomme, en sucre, et en un acide d’une nature particulie`re, par le moyen de l’acide sulfurique; conversion de la meˆme substance ligneuse en ulmine par la potasse. Ann. Chim. 1819, 12, 172–195. Payen, A. Me´moire sur la composition du tissu propre des plantes et du ligneux. Compt. Rend. 1838, 7, 1052–1056. Willsta¨tter, R.; Zechmeister, L. Zur Kenntnis der Hydrolyse von cellulose, I. Be 1913, 46, 2401–2412. Staudinger, H. Die Chemie der hochmolekularen organischen Stoffe im Sinne der Kekule`schen Strukturlehre. BER 1926, 59, 3019–3043. Irvine, J.C.; Hirst, E.L. The constitution of polysaccharides: Part VI. The molecular structure of cotton cellulose. J. Chem. Soc. 1923, 123, 518–532. Freudenberg, K.; Braun, E. Methylcellulose. Mitt. Lignin Cellulose Ann. 1928, 5 (460), 288–304. Charlton, W.; Haworth, W.N.; Peat, S. A revision of the structural formula of glucose. J. Chem. Soc., 1926; 89–101. Haworth, W.N. Revision of the structural formula of dextrose. Nature 1925, 116, 430. Haworth, W.N. The structure of carbohydrates. Helv. Chim. Acta 1928, 11, 534–548. Chu, S.S.C.; Jeffrey, G.A. The refinement of the crystal structures of b-D-glucose and cellobiose. Acta Crystallogr. 1968, 24, 830–838. Pe´rez, S.; Gautier, C.; Imberty, A. Oligosaccharide conformations by diffraction method. In Oligosaccharides in Chemistry and Biology; Ernst, B., Hart, G., Sinay, P., Eds.; Wiley/VCH, 2000; 969–1001. Philipp, B.; Linow, K.J. Untersuchungen zur Kettenlangendifferenz zwischen Nitrat- und Cuoxam-DP der Cellulose and ihrer A¨nderung im Viskoseprozelb. Papier 1960, 20, 649–657. Mark, R.E. Adhesion in cellulosic and wood-based composites. In Molecular and Cell Wall Structure of Wood; Oliver, J.F., Ed.; Plenum Press: New York, 1981; 7–51. Marx-Figini, M. U¨ber die Kinetik der Biosynthese der Cellulose in der Baumwolle. Papier 1964, 18, 546–549. Hermans, P.H.; Weidinger, A. X-ray studies on the crystallinity of cellulose. J. Polym. Sci. 1949, 4, 135–144. Fengel, D. Characteristics of cellulose by deconvoluting the OH valency range in FTIR spectra. Holzforschung 1992, 46, 283–288. Howsmon, J.A.; Sisson, W.A. High polymers, structure and properties of cellulose fibers: B. Submicroscopic structure. In Cellulose and Cellulose Derivatives, Part I; Ott, E., Spurlin, H.M., Eds.; Interscience: New York, 1963; Vol. V, 231–346. Isogai, A. Allomorphs of cellulose and other polysaccharides. In Cellulosic Polymers, Blends and Composites; Gilbert, R.D., Ed.; Hanser Publishing: Munich, 1994; 1–24. Atalla, R.H.; VanderHart, D.L. Native cellulose: a composite of two distinct crystalline forms. Science 1984, 223, 283–285. Chanzy, H.; Imada, K.; Vuong, R. Electron diffraction from the primary wall of cotton fibers. Protoplasma 1978, 94, 299–306. Chanzy, H.; Imada, K.; Mollard, A.; Vuong, R.; Barnoud, F. Crystallographic aspects of sub-elementary cellulose fibrils occurring in the wall of rose cells cultured in vitro. Protoplasma 1979, 100, 303–316.
35. Ambronn, H. U¨ber das Zusammenwirken von Sta¨bchendoppelbre-chung und Eigendoppelbrechung I. Kolloid-Z. 1916, 18, 90–97. 36. Ambronn, H. U¨ber das Zusammenwirken von Sta¨bchendoppelbre-chung und Eigendoppelbrechung II. Kolloid-Z. 1916, 18, 273–281. 37. Kubo, T. Untersuchungen U¨ber die Umwandlung von Hydratcellulose in natu¨rliche Cellulose: VII. Die Kristallstruktur des Umwandlungs-produktes sowie eines ho¨chst orientierten natu¨rlichen Cellulosepra¨parates. Z. Phys. Chem. 1940, 187, 297–312. 38. Wellard, H.J. Variation in the lattice spacing of cellulose. J. Polym. Sci. 1954, 13, 471–476. 39. Meyer, K.H.; Mark, H. U¨ber den Bau des krystallisierten Anteils der Cellulose. Ber 1928, 61, 593–614. 40. Gardner, K.H.; Blackwell, J. The structure of native cellulose. Biopolymers 1974, 13, 1975–2001. 41. Sarko, A.; Muggli, R. Packing analysis of carbohydrates and polysaccharides: III. Valonia cellulose and cellulose II. Macromolecules 1974, 7, 486–494. 42. Claffey, W.; Blackwell, J. Electron diffraction of Valonia cellulose. A quantitative interpretation. Biopolymers 1976, 15, 1903–1915. 43. Fischer, D.G.; Mann, J. Crystalline modification of cellulose: Part VI. Unit cell and molecular symmetry of cellulose I. J. Polym. Sci. 1960, 62, 189–194. 44. Nieduszynski, I.A.; Preston, R.D. Crystallite size in natural cellulose. Nature 1970, 225, 273–274. 45. VanderHart, D.L.; Atalla, R.H. In Cellulose: Structure, Modification and Hydrolysis; Young, R.A., Rowell, R.M., Eds.; New York: Wiley Interscience, 1986; 88–118. 46. Belton, P.S.; Tanner, S.F.; Cartier, N.; Chanzy, H. High resolution solid state 13C NMR spectroscopy of Tunicin, an animal cellulose. Macromolecules 1989, 22, 1615–1617. 47. Sugiyama, J.; Persson, J.; Chanzy, H. Macromolecules. Combined infrared and electron diffraction study of the polymorphism of native celluloses. Macromolecules 1991, 24, 2461–2466. 48. VanderHart, D.L.; Atalla, R.H. Further carbon-13 NMR evidence for the coexistence of two crystalline forms in native celluloses. ACS Symp. Ser. 1987, 340, 88–118. 49. Atalla, R.H.; Whitmore, R.E.; VanderHart, D.L. A highly crystalline a cellulose from Rhizoclonium hieroglyphicum. Biopolymers 1985, 24, 421–423. 50. Chanzy, H.; Henrissat, B.; Vincendon, M.; Tanner, S.; Belton, P.S. Solid-state 13C-NMR and electron microscopy study on the reversible cellulose I to cellulose IIII transformation in Valonia. Carbohydr. Res. 1987, 160, 1–11. 51. Hirai, A.; Horii, F.; Kitamaru, R. Transformation of native cellulose crystals from cellulose Ih to cellulose Ia through solid-state chemical reactions. Macromolecules 1987, 20, 1440–1442. 52. Tanahashi, M.; Goto, T.; Horii, F.; Hirai, A.; Higuchi, T. Characterization of steam-exploded wood: III. Transformation of cellulose crystals and changes of crystallinity. Mokuzai Gakkaishi 1989, 35, 654–662. 53. Honjo, G.; Watanabe, M. Examination of cellulose fibre by the low-temperature specimen method of electron diffraction and electron microscopy. Nature 1958, 181, 326–328. 54. Marrinan, H.J.; Mann, J. Infrared spectra of the crystalline modifications of cellulose. J. Polym. Sci. 1956, 21, 301–311. 55. Mann, J.; Marrinan, H.J. Crystalline modifications of cellulose: Part II. A study with plane-polarized infrared radiation. J. Polym. Sci. 1958, 32, 357–370. 56. Wiley, J.H.; Atalla, R.H. Bands assignments in the Raman spectra of celluloses. Carbohydr. Res. 1987, 160, 113–129. 57. Imai, T.T.; Sugiyama, J.; Itoh, T.; Horii, F. Almost pure Ia
13.
14.
15. 16. 17. 18. 19. 20. 21. 22. 23. 24.
25.
26. 27. 28. 29. 30.
31. 32. 33. 34.
Pe´rez and Mazeau
66
58.
59.
60. 61. 62.
63. 64. 65. 66. 67.
68.
69. 70.
71.
72. 73. 74.
75. 76. 77. 78.
cellulose in the cell wall of Glaucocystis. J. Struct. Biol. 1999, 127, 248–257. Sugiyama, J.; Vuong, R.; Chanzy, H. Electron diffraction study on the two crystalline phases occurring in native cellulose from an algal cell wall. Macromolecules 1991, 24, 4168–4175. Koyama, M.; Helbert, W.; Imai, T.; Sugiyama, J.; Henrissat, B. Parallel-up structure evidences the molecular directionality during biosynthesis of bacterial cellulose. Proc. Natl. Acad. Sci. USA 1997, 94, 9091–9095. Heiner, A.P.; Sugiyama, J.; Teleman, O. Crystalline cellulose Ia and Ih studied by molecular dynamics simulations. Carbohydr. Res. 1995, 273, 207–223. Aabloo, A.; French, A.D.; Mikelsaar, R.H.; Perstin, A. Studies of the crystalline native celluloses using potentialenergy calculations Cellulose 1995, 1, 161–168. Kroon-Batenburg, L.M.J.; Bouma, B.; Kroon, J. Stability of cellulose structures studied by MD simulations. Could mercerized cellulose II be parallel? Macromolecules 1996, 29, 5695–5699. Vietor, R.J.; Mazeau, K.; Lakin, M.; Pe´rez, S. A priori crystal structure prediction of native celluloses. Biopolymers 2000, 54, 342–354. Simon, I.; Scheraga, H.A.; Manley, R.St.J. Structure of cellulose: 2. Low energy crystalline arrangements. Macromolecules 1988, 21, 990–998. Finkendstadt, V.L.; Millane, R.P. Crystal structure of Valonia cellulose Ih. Macromolecules 1998, 31, 7776– 7783. Nishiyama, Y.; Isogai, A.; Isogai, O.; Mu¨ller, T.M.; Chanzy, H. Intracrystalline deuteration of native cellulose. Macromolecules 1999, 32, 2078–2081. Nishiyama, Y.; Okano, T.; Langan, P.; Chanzy, H. High resolution neutron fibre diffraction data on hydrogenated and deuterated cellulose. Int. J. Biol. Macromol. 1999, 26, 279–283. Nishiyama, Y.; Langan, P.; Chanzy, H. Crystal structure and hydrogen-bonding system in cellulose Ih from synchrotron X-ray and neutron fiber diffraction. J. Am. Chem. Soc. 2002, 124, 9074–9082. Marechal, Y.; Chanzy, H. The hydrogen bond network in Ibeta cellulose as observed by infrared spectrometry. J. Mol. Struct. 2000, 523, 183–196. Atalla, R.H. Celluloses. In Comprehensive Natural Chemistry, Carbohydrates and Their Natural Derivatives Including Tanins, Cellulose and Related Lignins; Pinto, B.M., Ed.; Elsevier: Cambridge, 1999; Vol. 3, 529–598. Sugiyama, J.; Vuong, R.; Chanzy, H. Electron diffraction study of the two crystalline phases occurring in native cellulose from an algal cell wall. Macromolecules 1991, 24, 4168–4175. Wada, M.; Sugiyama, J.; Okano, T. Native cellulose on the basis of the two crystalline phase (Ia/Ih) system. J. Appl. Polym. Sci. 1993, 49, 1491–1496. Andress, K.R. The X-ray diagram of mercerized cellulose. Zietschrift Plysikali. Sohe Chem. Abstr., B 1929, 4, 190– 201. Ahmed, A.U.; Ahmed, U.; Aslam, J.; Butt, N.M.; Khan, Q.H.; Atta, M.A Neutron diffraction and studies of the unit cell of cellulose: II. Polymer letters (edition 14). J. Polym. Sci. 1976; 561–564. Kolpak, F.J.; Blackwell, J. Determination of the structure of cellulose II. Macromolecules 1976, 9, 273–278. Nyburg, S.C. X-ray analysis of organic structures. Fibrous Macromol. Subst. 1961; 302–314. Kuga, S.; Takagi, S.; Brown, R.M.J. Native folded-chain cellulose II. Polymer. 1993, 34, 3293–3297. Stipanovich, A.J.; Sarko, A. Packing analysis of carbohy-
79. 80.
81.
82.
83. 84. 85.
86. 87.
88. 89. 90. 91.
92. 93. 94. 95. 96.
97. 98.
drates and polysaccharides: 6. Molecular and crystal structure of regenerated cellulose II. Macromolecules 1976, 9, 851–857. Poppleton, B.J.; Mathieson, A. McL, crystal structure of hD-cellotetraose and its relationship to cellulose. Nature 1968, 219, 1046–1049. Gessler, K.; Krauss, N.; Steiner, T.; Betzel, C.; Sarko, A.; Saenger, W. h-D-celloteraose hemihydrate as a structural model for cellulose: II. An X-ray diffraction study. J. Am. Chem. Soc. 1995, 17, 11397–11406. Raymond, S.; Heyraud, A.; Qui, A.; Kvick, H. Crystal and molecular structure of h-D-cellotetraose hemihydrate as a model of cellulose II. Macromolecules 1995, 28, 2096–2100. Langan, P.; Nishiyama, Y.; Chanzy, H. A revised structure and hydrogen bonding system in Cellulose II from a neutron fiber diffraction analysis. J. Am. Chem. Soc. 1999, 121, 9940–9946. Langan, P.; Nishiyama, Y.; Chanzy, H. The X-ray structure of mercerized cellulose II at 1 A resolution. Biomacromolecules 2001, 2, 410–416. Sarko, A. What is the crystalline structure of cellulose? Tappi 1978, 61, 59–61. Sugiyama, J.; Okano, T. Electron microscopic and X-ray diffraction study of cellulose IIII and cellulose I. Cellulose and Wood: Chemistry and Technology, Proceedings of the Tenth Cellulose Conference; 1989; 119–127. Roche, E.; Chanzy, H. Electron microscopy study of the transformation of cellulose I into cellulose IIII in Valonia. Macromolecules 1981, 3, 201–206. Sarko, A.; Southwick, J.; Hayashi, J. Packing analysis of carbohydrates and polysaccharides: 7. Crystal structure of cellulose III, and its relationship to other cellulose polymorphs. Macromolecules 1976, 9, 857–863. Bule´on, A.; Chanzy, H. Single crystals of cellulose IVII. Preparation and properties. J. Polym. Sci. 1980, 18, 1209– 1217. Gardiner, E.S.; Sarko, A. Packing analysis of carbohydrates and polysaccharides: 16. The crystal structures of cellulose IVI and IVII. Can. J. Chem. 1985, 63, 173–180. Okano, T.; Sarko, A. Mercerization of cellulose: II. Alkalicellulose intermediates and a possible mercerization mechanism. J. Appl. Polym. Sci. 1985, 30, 325–332. Hayashi, J.; Yamada, T.; Shimizu, Y.-L. Memory phenomenon of the original crystal structure in allomorphs of Na-cellulose, 77-102. In Cellulose and Wood: Chemistry and Technology; Schuerch, C., Ed.; Wiley: New York, 1989. Okano, T.; Sarko, A. Mercerization of cellulose I. X-ray diffraction evidence for intermediate structures. J. Appl. Polym. Sci. 1984, 29, 4175–4182. Nishimura, H.; Okano, T.; Sarko, A. Mercerization of cellulose: 5. Crystal and molecular structure of Nacellulose I. Macromolecules 1991a, 24, 759–770. Nishimura, H.; Okano, T.; Sarko, A. Mercerization of cellulose: 6. Crystal and molecular structure of Nacellulose I. Macromolecules 1991b, 24, 771–778. Revol, J.F.; Goring, D.A.I. Directionality of the fiber c-axis of cellulose crystallites in microfibrils of Valonia ventricosa. Polymer 1983, 24, 1547–1550. Dinand, E.; Vignon, M.; Chanzy, H.; Heux, L. Mercerization of primary wall cellulose and its implication for the conversion of cellulose I!cellulose II. Cellulose 2002, 9, 3311–3314. Kratky, O.; Mark, H. Zur Frage der individuellen Cellulosemicellen. Z. Phys. Chem., B 1937, 36, 129–139. Preston, R.D.; Nicolai, E.; Reed, R.; Mallard, A. Electronmicroscopic study of cellulose in the wall of Valonia ventricosa. Nature 1948, 162, 665–667.
Conformations, Structures, and Morphologies of Celluloses 99. Frey-Wyssling, A.; Miihlethaler, K.; Wyckoff, R.W.G. Mikrofibrillenbau der pflanzlichen Zellwa¨nde. Experientia 1948, 4, 475–476. 100. Revol, J.F. Change of the d spacing in cellulose crystals during lattice imaging. J. Mater. Sci. Lett. 1985, 4, 1347– 1349. 101. Sugiyama, J.; Harada, H.; Fujiyoshi, Y.; Uyeda, N. High resolution observations of cellulose microfibrils. Mokuzai Gakkaishi 1985, 30, Sugiyama, J.; Harada, H.; Fujiyoshi, Y.; Uyeda, N. Observations of cellulose microfibrils in Valonia macrophysa by high resolution electron microscopy. Mokuzai Gakkaishi 1985, 31, 61–67. 102. Marchessault, R.H. Cellulosics as advanced materials. In Cellulose and Wood: Chemistry and Technology; Schuerch, C., Ed.; Wiley: New York, 1989; 1–2. 103. Meyer, K.H.; Misch, L. Position des atomes dans le nouveau module spatial de la cellulose. Helv. Chim. Acta 1937, 20, 232–244. 104. Colvin, J.R. Oxidation of cellulose microfibril segments by alkaline silver nitrate and its relation to the fine structure of cellulose. J. Appl. Polym. Sci. 1964, 8, 2763–2774. 105. Colvin, J.R. Tip-growth of bacterial cellulose microfibrils and its relation to the crystallographic fine structure of cellulose. J. Polym. Sci. 1966, 4, 747–754. 106. Kuga, S.; Brown, R.M.J. Silver labelling of the reducing ends of bacterial cellulose. Carbohydr. Res. 1988, 180, 345– 350. 107. Hieta, K.; Kuga, S.; Usuda, M. Electron staining of reducing ends evidences a parallel-chain structure in Valonia cellulose. Biopolymers 1984; 1807–1810. 108. Maurer, A.; Fengel, D. Parallel orientation of the molecular chains in cellulose I and cellulose II deriving from higher plants. Holz Roh-Werkst. 1992, 50, 493. 109. Chanzy, H.; Henrissat, B. Unidirectional degradation of Valonia cellulose microcrystals subjected to cellulose action. FEBS Lett. 1985, 184, 285–288. 110. Sugiyama, J.; Harada, H.; Fujiyoshi, Y.; Uyeda, N. Lattice imaging from ultrathin sections of cellulose microfibrils in the cell wall of Valonia macrophysa. Planta 1985, 166, 161– 168. 111. Sakurada, L.; Nukushina, Y.; Ito, T. Experimental determination of the elastic modulus of crystalline regions in oriented polymers. J. Polym. Sci. 1962, 57, 651–660. 112. Dufresne, A.; Kellerhals, M.B.; Witholt, B. Transcrystallization in Mc1-PHAs/cellulose whiskers composites. Macromolecules 1999, 32, 7396–7400. 113. Heux, L.; Dinand, E.; Vignon, M.R. Structural aspects in ultrathin cellulose microfibrils followed by 13C CP-MAS NMR. Carbohydr. Polym. 1999, 40, 115–124. 114. Liang, C.Y.; Marchessault, R.H. Infrared spectra of crystalline polysaccharides: I. Hydrogen bonds in native celluloses. J. Polym. Sci. 1959, 37, 385–395. 115. Tsuboi, M. Infrared spectrum and crystal structure of cellulose. J. Polym. Sci. 1957, 25, 159–171. 116. Rowland, S.P.; Roberts, E.J.; Wade, C.P. Selective accessibilities of hydroxyl groups in the microstructure of cotton cellulose. Text. Res. J. 1969, 39, 530–542. 117. Rowland, S.O.; Roberts, E.J. The nature of accessible surfaces in the microstructure of native cellulose. J. Polym. Sci., Part A 1972, 10, 2447–2461. 118. Rowland, S.P.; Roberts, E.J. Disposition of D-glucopyranosyl units on the surfaces of crystalline elementary fibrils of cotton cellulose. J. Polym. Sci., Polym. Chem. Ed. 1972, 10, 867–879. 119. Rowland, S.P.; Howley, P.S. Hydrogen bonding on accessible surfaces of cellulose from various sources and relationship to order within crystalline regions. J. Polym. Sci., Part A Polym. Chem. 1988, 26, 1769–1778.
67 120.
Rowland, S.P.; Howley, P.S. Structure in ‘‘amorphous regions,’’ accessible segments of fibrils, of the cotton fiber. Text. Res. J. 1988, 58, 96–101. 121. Verlhac, C.; Dedier, J.; Chanzy, H. Availability of surface hydroxyl groups in Valonia and bacterial cellulose. J. Polym. Sci., Part A Polym. Chem. 1990, 28, 1171–1177. 122. Tasker, S.; Badyal, J.P.S.; Backson, S.C.E.; Richards, R.W. Hydroxyl accessibility in celluloses. Polymer. 1994, 35, 4717–4721. 123. Baker, A.A.; Helbert, W.; Sugiyama, J.; Miles, M.J. Highresolution atomic force microscopy of native Valonia cellulose I microcrystals. J. Struct. Biol. 1997, 119, 129–138. 124. Baker, A.A.; Helbert, W.; Sugiyama, J.; Miles, M.J. Surface structure of native cellulose microcrystals by AFM: Part 1. Scanning tunneling microscopy/spectroscopy and related techniques. Appl. Phys., A Mater. Sci. Process., A 1998, 66 (Supplement), S559–S563. 125. Baker, A.A.; Helbert, W.; Sungiyama, J.; Miles, M.J. New insight into cellulose structure by atomic force microscopy shows the Ia crystal phase at near-atomic resolution. Biophys. J. 2000, 79, 1139–1145. 126. Hanley, S.J.; Giasson, J.; Revol, J.F.; Gray, D.G. Atomic force microscopy of cellulose microfibrils: comparison with transmission electron microscopy. Polymer. 1992, 33, 4639–4642. 127. Kuutti, L.; Peltonen, J.; Pere, J.; Teleman, O. Identification and surface structure of crystalline cellulose studied by atomic force microscopy. J. Microsc. 1995, 178, 1–6. 128. Newman, R.H.; Hemmingson, J.A. Carbon-13 NMR distinction between categories of molecular order and disorder in cellulose. Cellulose (London) 1995, 2, 95–110. 129. Heux, L.; Dinand, E.; Vignon, M.R. Structural aspects in ultrathin cellulose microfibrils followed by 13C CP-MAS NMR. Carbohydr. Polym. 1999, 40 (2), 115–124. 130. Woodcok, S.; Henrissat, B.; Sugiyama, J. Docking of Congo red to the surface of crystalline cellulose using molecular mechanics. Biopolymers 1995, 36, 201–210. 131. Houtman, C.; Atalla, R.J. Cellulose–lignin interactions: a computational study. Plant Physiol. 1995, 107, 977–984. 132. Heiner, A.P.; Teleman, O. Interface between monoclinic crystalline cellulose and water: breakdown of the odd/even duplicity. Langmuir 1997, 13, 511–518. 133. Heiner, A.P.; Kuutti, L.; Teleman, O. Comparison of the interface between water and four surfaces of native crystalline cellulose by molecular dynamics simulations. Carbohydr. Res. 1998, 306, 205–220. 134. Biermann, O.; Hadicke, E.; Koltzenburg, S.; MullerPlathe, F. Hydrophilicity and lipophilicity of cellulose crystal surfaces. Angew. Chem., Int. Ed. 2001, 40, 3822– 3825. 135. Mazeau, K.; Vergelati, C. Atomistic modeling of the absorption of benziphenone onto cellulosic surfaces. Langmuir 2001, 18, 1919–1927. 136. Chanzy, H.; Henrissat, B.; Vuong, R. Gold labelling of 1,4h-D-glucan cellobiohydrolase absorbed on cellulose substrates. FEBS Lett. 1984, 172, 193–197. 137. Gilkes, N.R.; Kilburn, D.G.; Miller, R.C.; Warren, R.A.J.; Sugiyama, J.; Chanzy, H.; Henrissat, B. Visualization of the adsorption of a bacterial endo-h-1,4-glucanase and its isolated cellulose-binding domain to crystalline cellulose. Int. J. Biol. Macromol. 1993, 15, 347–351. 138. Lehtio, J.; Sugiyama, J.; Gustavsson, M.; Fransson, L.; Linder, M.; Teeri, T.T. The binding specificity of family 1 and family 3 cellulose binding modules. PNAS 2003, 100, 484–489. 139. Jurasek, L. Experimenting with virtual lignins. ACS Symp. Ser. 1998, 697 (Lignin and Lignan Biosynthesis), 276– 293.
Pe´rez and Mazeau
68 140.
Faulon, J.L.; Hatcher, P.G. Is there any order in the structure of lignin? Energy Fuels 1994, 8, 402–407. 141. Radotic, K.; Radotic; Simic-Krstic, J.; Jeremic, M.; Trifunovic, M. A study of lignin formation at the molecular level by scanning tunneling microscopy. Biophys. J. 1994, 66, 1763–1767. 142. Lichtenegger, H.; Mu¨ller, M.; Paris, O.; Riekel, C.; Fratzl, P. Imaging of the helical arrangement of cellulose fibrils in wood by synchrotron X-ray microdiffraction. J. Appl. Crystallogr. 1999, 32, 1127–1133. 143. McCann, M.; Weels, B.; Roberts, K. Direct visualization of cross-links in the primary cell walls. J. Cell. Sci. 1990, 96, 323–334. 144. Brown, M.R.; Saxena, I.M. Jr. Cellulose biosynthesis: a model for understanding the assembly of biopolymers. Plant Physiol. Biochem. 2000, 38, 57–67. 145. Chandrasekaran, R. Molecular architecture of polysaccharide helices in oriented fibers. Adv. Carbohydr. Chem. Biochem. 1997, 52, 311–439. 146. French, A.D.; Kelterer, A.-M.; Johnson, G.P.; Dowd, M.K.; Cramer, C.J. Constructing and evaluating energy
147.
148.
149. 150.
151.
surfaces of crystalline disaccharides. J. Mol. Graph. Modell. 2000, 18, 95–107. Raymond, S.; Henrissat, B.; Tran-Qui, D.; Kvick, A.; Chanzy, H. The crystal structure of methyl h-cellotrioside monohydrate 0.25 ethanolated and its relationship to cellulose II. Carbohydr. Res. 1995, 277, 209–229. Rencurosi, A.; Ro¨hrling, J.; Pauli, J.; Potthast, A.; Ja¨ger, C.; Pe´rez, S.; Kosma, P.; Imberty, A. Polymorphism in the crystal structure of the cellulose fragment analogue methyl 4-O-methyl-h-D-glucopyranosyl-(1–4)-h-D-glucopyranoside. Angew. Chem., Int. Ed. 2002, 22, 4277–4281. Ham, J.T.; Williams, D.G. The crystal and molecular structure of methyl h-cellobioside methanol. Acta Crystallogr., B 1970, 26, 1373–1383. Nishiyama, Y.; Sugiyama, J.; Chanzy, H.; Langan, P. Crystal structure and hydrogen bonding system in cellulox Ia from synchrotron x-ray and neutron fiber diffraction. J. Am. Chem. Soc. 2003, 125, 16300–16306. Sassi, J.F. Etude ultrastructurale de l’ace´tylation de la cellulose. Application a` la preˆparation de nanocomposites, The`se de doctorat de l’Universite´ Joseph Fourier, 1995.
3 Hydrogen Bonds in Cellulose and Cellulose Derivatives Tetsuo Kondo Kyushu University, Fukuoka, Japan
I. HYDROGEN BONDS IN CELLULOSE The native biopolymer assembly has been shown to be a complex process involving two separate but integrated steps of polymerization and crystallization [1,2]. In particular, cellulose has shown to be assembled by a macromolecular complex of enzymes located on the cell surface. Nature has designed an efficient system for regulating the molecular weight, crystallinity, size, and shape of the nanostructure of cellulose (called cellulose microfibrils). Then the microfibrils are self-assembled to form cell walls maintaining tree-frame structure. In this manner, cellulose molecules biosynthesized at angstrom scale assemble to be microfibrils at nanoscale, and the microfibrils assemble to be cell walls at micronscale, then they scale up with growing (Fig. 1). Hydrogen bonds are no doubt a major interaction to stabilize this hierarchical architecture of higher plants. Therefore considering hydrogen bonds of cellulose requires in your mind a picture of the size (angstrom, nano, or micron) of the subject that you are looking at. First, cellulose is considered as a single molecule (primary or chemical structure): cellulose owns an extended structure with a 21 screw axis composed of the h-1,4 glucosidic linkages between anhydroglucose units. Thus it would be natural to accept the dimer called ‘‘cellobiose’’ as a repeating unit. The present three kinds of hydroxyl groups within an anhydroglucose unit exhibit different polarities, which contribute to the formation of various kinds of inter- and intramolecular hydrogen bonds among secondary OH at the C-2, secondary OH at the C-3, and primary OH at the C-6 position (Fig. 2). In addition, all the hydroxyl groups are bonded to a glucopyranose ring equatorially. This causes the appearance of hydrophilic site parallel to the ring plane. On the contrary, the CH groups are bonded to a glocopyranose ring axially, resulting in a hydrophobic site perpendicular to the ring as shown in Fig. 3. These effects lead to the
formation of hydrogen bonds in parallel direction to a glucopyranose ring, and to van der Waals’ interaction perpendicular to the ring. Another important point for the hydroxyl groups is the type of hydroxymethyl conformation at the C-6 position, because the conformation of C(5)–C(6) and the resulting interactions including inter- and intramolecular hydrogen bonds in the present cellulose structure may differ from that in crystallites as described in the following section, and it is also assumed to make up the extent of crystallization, as well as the final morphology of cellulose [3–5]. In the noncrystalline regions, the rotational position of hydroxymethyl groups at the C-6 position may be considered as indeterminate or totally nonoriented, whereas all of those are identical in the crystallites. Therefore it was important to confirm the type of O(6) rotational position with respect to the O(5) and C(4) in a h-glucan chain, employing CP/MAS 13C NMR [6]. The type of hydroxymethyl conformations, gauche–trans (gt), trans–gauche (tg), or gauche–gauche (gg) at the C-6 positions in carbohydrates is shown in Fig. 4. In the gt conformation, hydroxyl groups (OH) at the C-6 position locate at the opposite side to OH at the neighboring C-2 position, and thus they are supposed to form intermolecular hydrogen bonds with the neighbors, whereas tg conformation may provide intramolecular hydrogen bonds engaged between OH groups at the C-2 and C-6 positions. As for the noncrystalline states, they are considered as the gg conformation. As described above, the difference in polarity among hydroxyl groups and hydroxymethyl conformation at the C-6 position in relation to equatorial bonding of them to an anhydroglucose ring is strongly attributed to inter- and intramolecular hydrogen bonds of cellulose. Further, the hydrogen bonding patterns in cellulose are considered as one of the most influential factors on the physical properties of cellulose and its derivatives shown in Fig. 2. This issue will be treated later in this chapter. 69
70
Kondo
Figure 1 Hierarchical system of cellulose self-assembly.
Of course, cellulosic fibers and materials are made of inter- and intramolecular hydrogen bonds, and turning to the molecular structure of cellulose, intramolecular hydrogen bonds are primarily to be employed as a most influential interaction to the molecule. Cellulose is supposed to have at most two different intramolecular hydrogen bonds, which are between the OH-3 and adjacent ring O-5V and between the OH-6 and OH-2V when the hydroxymethyl conformation at the C-6 position is tg (Fig. 5) [7–11]. The intramolecular hydrogen bonds influence first on the molecular main chain stiffness. Is the main chain for each cellulose single molecule that seems to be stiff really stiff ? For this question, extensive studies of solution properties and liquid crystalline properties for cellulose and cellulose derivatives have been carried out. At the moment it is explained that the main chain for each cellulose molecule is not so stiff, and rather the molecule itself is a semiflexible one in which the worm-like chain model by Heine et al. [12] can be well applied to [13–15]. Therefore one single molecule is considered relatively mobile. Only a single molecule, however, cannot exist in normal states. The molecules are mutually influenced and interacted with each other. There may be two stabilizing ways for each molecule, depending on the initial step. One is that after a single molecule interacts with other molecules, then each molecule compensates the potential energy to be stabilized. Another is that first the potential energy for each molecule is minimized and after the minimization, it starts interacting with each other by hydrogen bonding, van der Waals’ force, and dipole moment interaction. In any case, every single cellulose molecule interacts with each other. Therefore it becomes important to characterize the interaction that is engaged between molecules and further the relationship
Figure 2 A general idea on the correlation of basic characters for each hydroxyl group with physicochemical properties.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
Figure 3
71
Hydrophilic and hydrophobic nature in cellulose chemical structure.
between the interaction and physical properties of cellulose and the derivatives in order to anticipate both the physical and chemical characteristics of new cellulosic materials [16–28]. Among the interactions in cellulose, the hydrogen bonding interaction should be most frequently observed. Fig. 2 shows a general idea on the correlation of basic characters for each hydroxyl group with the physicochemical properties. Cellulose exhibits really versatile properties ranging from transformation of crystalline form to the regiochemical difference of the reactivity for the chemical derivatization and enzymatic hydrolysis. We have to distinguish the situation for the hydrogen bonds depending on
the state such as crystals, noncrystalline and amorphous solids, gels, liquid crystals, and solutions.
A. Hydrogen Bonds in Cellulose Crystals In this section, the object is up-scaled from a single molecule of cellulose up to a microfibril as a molecular assembled state. As shown in Fig. 6, after the biosynthesis of cellulose molecular chain, each single glucan chain starts associating with each other to self-assemble into a microfibril at a nanoscale (3.5–4.0 nm for wood microfibrils). Biosynthesis is an integrated step to form crystalline form of cellulose as a microfibril. The process mostly
Figure 4 Schematic diagram of the hydroxymethyl conformations at the C-6 position, namely, the orientation of the C6–O6 bond, gauche–trans (gt), trans–gauche (tg), or gauche–gauche (gg) with a cellobiose unit.
72
Kondo
Figure 5 Possible intramolecular hydrogen bonding formation in tg conformation of hydroxymethyl groups in cellulose.
produces highly crystalline domains, but not necessarily a perfect process to secrete a cellulose crystalline fiber. Therefore a cellulose fibril contains a certain amount of noncrystalline domains as illustrated in Fig. 6. About cellulose biosynthesis, there are many books from different viewpoints (see, for example, Ref. [29]). In this way, crystalline cellulose domain is an idealistic assembly of cellulose molecules in the biological system. Then hydroxyl groups equatorially bonded to the glucose ring become closer enough among neighboring h-glucan chains to form intermolecular hydrogen bonding. Therefore it would be of more importance to understand intermolecular interactions in crystalline cellulose. Crystalline cellulose has different crystalline forms from cellulose I to cellulose IV, and even in alkaline conditions it shows so-called alkali–cellulose crystals, which still gives a question as to the manner of existence. In each form, the chains have approximately the same
Figure 6
backbone conformation, with the two glucose residues repeating in approximately 1.03 nm. Recently, native cellulose (cellulose I) was found to be a composite of cellulose Ia and cellulose Ih crystalline forms by Atalla and VenderHart [30]. However, some of the crystalline structures such as cellulose IV are still in question so far. Therefore we only focus on conventional crystalline structure, cellulose I and cellulose II. In particular, for cellulose I, we will employ cellulose Ih, which is two-chain monoclinic [31] and is close to the proposed models on the basis of X-ray and electron diffraction data as well as chain packing energetics [32,33]. Thus we can easily understand the formation of hydrogen bonds using the models. On the other hand, because, to date, we cannot have pure cellulose Ia, it is still difficult to explain the hydrogen bonding formation for the cellulose Ia crystalline form. Just recently, a revised structure and a hydrogen bonding system in cellulose Ih [34] and cellulose II [35] have been proposed. In this section, the new insight as well as the previous one will be compared historically. Before getting into the details, we will confirm how to take the crystallographic axes (a, b, and c) and a certain angle, g, between the a–b axes. Now many people use the recent crystallographic rule, namely, c axis is a molecular axis, but still some researchers take b axis for the molecular chain axis. In fact, the number of researchers who use the recent crystallographic rule is increasing gradually. In this chapter, we will follow the recent rule. 1. Hydrogen Bonds in Native Cellulose (Cellulose I) The crystalline nature of cellulose was revealed almost a century ago when Nishikawa and Ono recorded the first X-ray diffraction patterns from fiber bundles originated
Crystalline and noncrystalline regions of cellulose microfibrils.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
from various plants [36]. Since then, in addition to X-ray, many powerful tools have appeared for investigating cellulose crystalline structures such as electron diffraction and microscope, FT-IR, Raman spectroscopy, and 13C CP/ MAS NMR. The development of high-resolution 13C solid-state NMR techniques in the 1980s has brought a new dimension to determining the crystal structure of cellulose. In fact, 13C CP/MAS NMR of highly crystalline cellulose samples such as Valonia showed the presence of two crystalline allomorphs (cellulose Ia and Ih) in cellulose I. However, FT-IR is still one of the best tools to study hydrogen bonding formation with consideration of the two-chain unit cell models (21 axis) [37]. In particular, not only FT-IR but also advanced FT-IR technique in combination with suitable attachments could provide us with further information on cellulose supermolecular structure. Many reports using IR analyses have appeared to date. Fengel analyzed the hydroxyl absorption bands by deconvoluted FT-IR spectra of celluloses [38–40]. Michell used the second-derivative mode in order to improve the FT-IR resolution [41–43]. The assignments for the hydroxyl frequencies had been established from the late 1950s to the early 1960s on the basis of the modified Meyer–Misch model [44–47]. In addition, the O–H stretching frequencies due to intra- and intermolecular hydrogen bonds in cellulose I were calculated [48]. Table 1 lists these reported band-assignments for native cellulose. To make an easy understanding of the hydrogen-bonding network, we will use the ab and bc projection of the unit cell for cellulose I (21 screw) originally proposed by Gardner and Blackwell [32] as shown in Fig. 7. This permits the formation of two intramolecular hydrogen bonds, OH-3: : :O5V and OH-
73
2: : : O6V, to give an even more rigid four-ring layer configuration. In these structures there is an intermolecular hydrogen bond, OH-6: : :O3 (Fig. 7C), linking the layers laterally, but no bonding between layers. In other words, there is no intermolecular hydrogen bonding along the (110) and (110) planes, but there is only one along the (200) plane as shown in Fig. 7A. Investigating hydrogen bonds in cellulose using IR was first performed by Marrinan and Mann [44,49], and then Liang and Marchessault [46,47] proceeded to assign the whole area of OH stretching frequencies in IR spectra for celluloses I and II. They used polarized IR measurements for oriented films having cellulose I or cellulose II crystalline structures and assigned some typical maxima for the OH regions of the IR spectra on the basis of the difference between the parallel and the perpendicular bands. Now let us take a look at Table 1 [46,48,50–52] and you would find that two intramolecular hydrogen bonds and an intermolecular hydrogen bond have already been assigned. Some experimental assignments correspond to the calculated wavenumbers [48]. In the 1980s, the crystalline dimorphism of native celluloses was found [30,53], and the two phases, cellulose Ia and Ih, have been considered to differ in their hydrogen bonding rather than in the conformation on the basis of Raman [51] and FT-IR [31,43] spectral data. According to Sugiyama et al. [52], a characteristic hydroxyl absorption band due to Ia crystalline phase is 3240 cm 1, whereas a band at 3270 cm 1 is due to Ih crystalline phase. There are a number of literatures reporting on the IR data of native cellulose [40–46,49,52,54]. Most of these studies give more or less complete lists of IR band assignments on the hydrogen bonding system. Most of these earlier IR studies,
Table 1 IR Assignments for OH Regions Reported in Native Cellulose
Frequency (cm 1) 3230–3310
Interpretation (Liang et al. 1959:L) (Ivanova et al. 1989:I) (Sugiyama et al. 1991:S)
Cellulose Ia (?) appeared in Valonia S: Cellulose Ia S: Cellulose Ih L: OH Inter H-bond OH Inter H-bond L&I: O(3)H–O(5) intra H-bond
3372 3405 3410–3460
OH Intra H-bond inter–O(3)H–O(5) L: OH Inter H-bond I: O(2)–O(6) Intra H-bond
3412 3429
Calculated wavenumbers (Tashiro et al. 1991)
I: O(6)H–O(3) Inter H-bond
3231 3240 3270 3305 3309 3340–3375
Interpretation by Raman (Wiley et al. 1987)
OH Intra H-bond O(2)–O(6)–inter Cellulose Ih (?) appeared in Ramie
74
Kondo
Figure 7 Proposed structure of cellulose I before the discovery of native cellulose allomorphs, Ia and Ih, in 1983 by Atalla and VanderHart [29]. (A) ab projection (looking along the chain axis); (B) bc projection; (C) hydrogen-bonding network in the sheet parallel to the bc plane. This figure is modified on the basis of the Gardner and Blackwell model [31].
however, were made before the discovery of the two crystalline phase system of cellulose. Thus a number of the earlier band assignments should be reevaluated in light of the two-phase system. Recently, Mare´chal and Chanzy [55] have reported the revised assignments of the IR bands in cellulose Ih from hydrothermally treated Valonia microfibrils. Their assignments are illustrated in Fig. 8. According to them, hydroxymethyl moieties were found adopting three conformations (a dominant one and two minor ones) allowing the formation of different hydrogen bonding on adjacent chains. Most probably, the primary hydroxyl groups (OH) that accept a hydrogen bond from the adjacent OH at the C-2 position were not the ones adopting the dominant conformation. However, there are still some questions remaining as OH bands due to different modes overlap with each other, causing difficulties in interpretation even in crystalline structures. The crystal and molecular structure of cellulose I need to be revised also in light of this dimorphism. This revision
requires data of pure Ia and Ih fibers. Recently, the revised data have been proposed using synchrotron and neutron diffraction for oriented fibrous samples from tunicate cellulose microcrystals [34]. The study proposed not only the revised Ih crystalline structure, but also the tg conformation of hydroxymethyl groups and the hydrogen bonding fashion. The hydrogen bonding scheme is represented schematically in Fig. 9: There is no hint of intersheet O–H– O hydrogen bonds in cellulose Ih, indicating that the cellulose sheets are held only by hydrophobic interactions and weak C–H–O bonds. Within the sheet, the intramolecular O3–O5 hydrogen bonds were well defined, whereas those corresponding O2–O6 hydrogen bonds were indicated in a variety of the fashion. 2. Hydrogen Bonds in Cellulose II Native cellulose can be easily transformed into cellulose II after an alkaline treatment at more than 18 wt.% and
Hydrogen Bonds in Cellulose and Cellulose Derivatives
75
Figure 8 Assignment of IR bands of cellulose Ih, with stretching bands drawn as two-headed arrows and bending bands of alcoholic groups as single-headed arrows. Assignments of bending bands to a particular alcohol group are tentative and may be the object of permutations between the three types of alcohols. Three conformations of hydroxymethyl groups at the C-6 position are displayed labeled I, II, and III. Conformations of II and III are deduced from conformation I by rotation of them around the C5–C6 bond. Conformation I represents at least 2/3 of the total conformations, conformation II (tg) less than 10%. Hydrogen bonds are supposed to be established by these primary alcohols on O atoms of other chains. For commodity hydroxyl groups at the C-2 position establishing weak hydrogen bonds is drawn with free OH groups [55].
subsequent washing thoroughly with distilled water. For cellulose II crystalline structure, some models have been proposed and they have defined the crystals as consisting of two antiparallel and crystallographically independent chains. The proposed structure has a monoclinic cell where the chains are aligned on the 21 screw axes. Both chains have equivalent backbone conformation but differ in the conformation of hydroxymethyl groups proposed by two groups, Kolpak and Blackwell [56] and Stipanovic and Sarko [57]. Their antiparallel model for cellulose II is shown in Fig. 10. The ab projection shows that the chains have approximately the same orientation about their axes and are stacked along the short ab diagonal (Fig. 10B). These stacks will be stabilized by hydrophobic (van der Waals) forces, more so than between the sheet in native cellulose. The relative stagger of the chains is 0.216c, again close to the quarter-stagger position. The refinement has led to different conformations of the –CH2OH groups on the center and corner chains. Adjacent center chains along the a axis are shown in Fig. 10C. The –CH2OH groups are oriented like those in native cellulose, so as to allow the formation of a second intramolecular hydrogen bond OH2V: : :OH-6 and an intermolecular hydrogen bond OH6: : : OH-3 along the a axis. The sheet of corner chains is shown in Fig. 10D. Here the –CH2OH group is swung round so that it forms an OH-6: : :OH-2 intermolecular hydrogen bond. Intramolecular bonding for OH-2 is now not possible, and this group forms another intermolecular
hydrogen bond OH-2: : :OH-2V to the next chain along the long ab diagonal. This bond is shown in Fig. 10E and is indicated by the dashed lines in Fig. 10A. This extra intermolecular bonding is a major difference between cellulose II and native cellulose and probably goes a long way to explain the higher stability of the regenerated form [58]. Table 2 lists the experimental IR assignments [47] and
Figure 9 Schematic representation of the hydrogen bonds in the origin (top) and center (bottom) sheets of cellulose Ih. Hydrogen bonds are represented by dotted lines. Only the oxygen atoms involved in hydrogen bonding have been labeled for clarity. (From Ref. 34.)
76
Kondo
Figure 10 Structure of cellulose II proposed by Kolpak and Blackwell [56]. (A) ac projection; (B) ab projection (- - - hydrogen bonds between center and corner chains); (C) hydrogen-bonding of the center chains; (D) hydrogen-bonding of the corner chains; (E) hydrogen-bonding between corner and center chains. This figure is modified on the basis of their model.
Hydrogen Bonds in Cellulose and Cellulose Derivatives Table 2 IR Assignments for OH Regions Reported in Cellulose II Frequency (cm 1) (Tashiro et al. 1991) 3175 3305 3308 3309 3315 3350 3374 3435 3447 3486 3488
Interpretation
Calculated wavenumbers (Marchessault et al. 1960)
OH stretching OH Inter H-bond
77
B. Hydrogen Bonds in Regioselectively Substituted Cellulose Derivatives in Solid-State Noncrystalline Films 1. Characterization Using FT-IR and Solid-State CP/MAS 13C NMR Spectra The formation of hydrogen bonds in cellulosics is considered as one of the most influential factors on the physical
OH Inter H-bond OH Inter H-bond OH Intra H-bond (Corner chain) ? OH Intra H-bond (center chain) OH stretching OH Intra H-bond (corner chain) OH Inter H-bond
calculated wavenumbers [48] for cellulose II. The model for the crystalline structure indicated the formation of intraand intermolecular hydrogen bonds for cellulose II. In this model, hydroxymethyl moieties are near gt conformation for the glycosyl residues located at the origin of the cell as opposed to tg conformation for those at the center chain. The model of cellulose II has been further investigated using h-cellotetraose hemihydrate and methyl h-cellotrioside monohydrate 0.25 ethanolate [59–62]. Their molecular configuration was also similar to that of the cellulose II model except in two main respects: all hydroxymethyl groups are in gt conformation and the sugar pucker was different for the two chains. In addition, the proposed hydrogen bonding schemes using oligosaccharides were significantly different from the previous ones. Recently, Langan et al. have reexamined the structure of cellulose II using a neutron fiber diffraction analysis [35]. In crystalline fibers of cellulose II, a 3-D network of hydrogen bonds exists. This new model as shown in Fig. 11 indicates a new substantially different hydrogen bonding network from previous proposals. In Fig. 11, intermolecular hydrogen bonds are O2-D-O6 in sheets containing only origin molecules and O6-D-O2 in sheets containing only center molecules. In the sheets containing both center and origin molecules there are O6-D-O6 and O2-D-O2 intermolecular hydrogen bonds. The former has minor components involving O5 and O3 as acceptors. Intramolecular hydrogen bonds are O3-D-O5 in each molecule with a minor component involving O6 as acceptor. However, you would notice that there are still difficulties in the interpretation of reactivity, properties of cellulose in various forms, and transformation process of cellulose from one to the other as well as even crystalline structures, as OH groups with different modes overlap with each other.
Figure 11 A schematic representation of hydrogen bonds on cellulose II proposed by Langan et al. [35]. Only atoms involved in hydrogen bonds are represented by dotted lines.
78
Figure 12 The chemical structures of regioselectively substituted cellulose derivatives prepared in Ref. [67].
properties of not only cellulose itself but also its derivatives. The previous section explained the possible formation of hydrogen bonds in native cellulose and cellulose II crystalline structures. As for cellulose derivatives, they show either crystalline structure or noncrystalline structure, depending on the degree of substitution (DS) and the structural regularity or the distribution pattern of substituted units along the molecular chain. For cellulose derivatives we can use NMR spectroscopy to observe hydrogen-bonding engagements [63]. In this case, we can mostly use solution NMR as solid-state NMR still has a problem on the resolution for signal splitting. However, most of the investigations on hydrogen bonding formation in cellulose as a polymer have difficulties in interpreting the chemical shift for the same reason as those studies using IR spectroscopy. Therefore we had better simplify the formation of hydrogen bonds to be more easily analyzed if possible. How can we do this? Kondo and Gray developed the methods for synthesizing regioselectively substituted cellulose ethers, 2,3-di-O-, 6-O-, and tri-O-substituted cellulose derivatives [64–67] as shown in Fig. 12. As the hydroxyl groups should form controlled intra- and intermolecular hydrogen bonds particularly in regioselectively methylated celluloses, the cellulose derivatives are thought to be cellulose model compounds to investigate the relationships between formation of hydrogen bonds and physical properties of cellulose, as well as the cellulose derivatives. When the OH groups within the anhydroglucose units are blocked by methyl groups, it remains a question whether the pyranoglucose ring conformation still keeps the original shape (4C1 chair conformation) or not. To answer this question, it has already been reported [25] that the OH groups in the anhydroglucose units, despite being blocked by methyl groups, do not affect the structure of the glucose ring. In other words, blocking hydroxyls by methyl groups in
Kondo
cellulose can be useful in controlling the formation of hydrogen bonds without causing a resultant change in the glucose ring conformation. Thus the regioselectively methylated celluloses have been proven to be satisfactory model compounds for cellulose. In continuation, the formation of hydrogen bonds in the regioselectively substituted cellulose derivatives was characterized by FT-IR and solid-state CP/MAS 13C NMR spectra of the film samples [67]. Fig. 13 shows OH frequencies for film samples of typical regioselectively substituted cellulose ethers, namely, 2,3-di-O- and 6-Omethylcellulose (23MC and 6MC), compared with that of pure cellulose. They were all predominantly noncrystalline films with ca. 5-Am thickness prepared by casting from their dimethyl acetoamide (DMAc) solutions for methylated derivatives and the DMAc-LiCl cellulose solution for pure cellulose, respectively. Therefore we do not have to take into account specifically oriented intermolecular hydrogen bonds, differently from the crystalline samples. Thus we have only to consider the following hydrogen bonds for the above amorphous film samples: isotropic intermolecular hydrogen bonds and two different intramolecular hydrogen bonds, which are between the OH-3 and adjacent ring O-5V and between the OH-6 and OH-2V (Fig. 14A). Looking at the spectra in Fig. 13 under these assumptions, we will find that they exhibited characteristic band shapes in the OH stretching vibration regions. The shape of the 6-Omethylcellulose (6MC) having two OH groups in a unit is rather symmetric and sharp, compared with that of 2,3-diO-methylcellulose (23MC), which has one OH group per anhydroglucose unit. Generally, increasing the number of
Figure 13 IR spectra of noncrystalline film samples of (A) cellulose, (B) 2,3-di-O-, and (C) 6-O-methylcellulose derivatives in the region of OH stretching vibration.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
Figure 14 Schematic representation of possible hydrogen bonds in cellobiose units of (A) cellulose, (B) 2,3-di-O-, and (C) 6-O-substituted cellulose derivatives.
OH groups per unit should show the diversity of OH frequencies in IR spectra, and then the absorption band should become broader. In the present case, however, the appearance of OH band of 6MC, which has two OH groups per unit, is contradictory. This phenomenon appeared in other relationships between 6-O- and 2,3-diO-substituted cellulose derivatives with the same substituent [67]. It is assumed that the phenomenon is attributed mainly to the manner of formation of hydrogen bonds. Schematic representations of possible inter- and intramolecular hydrogen bonds in the cellobiose unit are shown in Fig. 14. Cellulose may possibly have two types of intramolecular hydrogen bonds and some intermolecular hydrogen bonds, depending on the phase. While the intermolecular hydrogen bonds are not specified, the two intramolecular hydrogen bonds are assumed to be either OH-3-OV5 or OH-6-OH-2V (Fig. 14A). In the 2,3-di-Osubstituted cellulose derivatives, the main reason for the broader OH bands due to the diversity of OH frequencies appears to be the formation of intermolecular hydrogen bonds associated with OH-6. In the case of 6-O-substituted cellulose, specific intramolecular hydrogen bonding formation, which makes the IR band of the OH region symmetric and sharper, may exist. Hydroxyl and ring ether (C-O-C) groups correspond to the hydrogen bonding donor and acceptor, respectively, which are common in
79
biological structures. When the donor group is cation-like or the acceptor group is anion-like, as in O–H+–O or O– H–O , strong and almost symmetrical hydrogen bonds are also observed [1]. Because in 2,3-di-O-substituted cellulose free OH groups at the C-6 position are comparatively flexible, intermolecular hydrogen bonds may be formed favorably. The OH groups may also form intramolecular hydrogen bonds with the ether oxygen at the adjacent C-2 position (Fig. 14B). Thus, mixture of the inter- and the intramolecular hydrogen bonds is considered to cause the broadening of the OH band in the IR spectra. On the other hand, two intramolecular hydrogen bonds may form in the 6-O-substituted cellulose derivatives as shown in Fig. 14C. The two intramolecular hydrogen bonds (O6HO-2V and 3-OH-O5V) have similar type of formation, which is between the OH group and the ether or acetal oxygen. Therefore the sharp and symmetric IR spectra of 6O-substituted cellulose derivatives in Fig. 15 indicate that the two intramolecular hydrogen bonding structures may give a similar OH absorption band, and intermolecular hydrogen bonding formation which broadens the OH band may be not significant. Furthermore, the strengths of the two hydrogen bonds may be almost equivalent, and hence both of the intramolecular hydrogen bonds between the OH and the ether oxygen appear at almost the same wave number around 3465 cm 1 in OH stretching frequencies of the IR bands. In another experiment [68], the curve fitting procedure was performed for the regions due to OH stretching vibration in the IR spectra of the noncrystalline films from 2,3-di-O-methylcellulose (2,3-di-O-MC) and 6-O-methylcellulose (6-O-MC). The results are shown in Fig. 16. The OH bands for 2,3-di-O-MC are resolved into two Lorentzian bands, sharper (3472 cm 1) and broad (3382 cm 1) ones; 6MC has one major Lorentzian OH absorption band (3460 cm 1) and a small subband (3270 cm 1). These bands may correspond to the presence of specific inter- and intramolecular hydrogen bonds involved in 2,3-di-O-MC and 6-O-MC as mentioned above. Thus the bands with peak positions at higher wavenumbers of 3460–3470 cm 1 for both 2,3-di-O-MC and 6-O-MC result in the assignments of the following intramolecular hydrogen bonds, because in general for cellulosic materials the intramolecular hydrogen bonds tend to appear at relatively higher wave numbers (3410–3460 cm 1 in cellulose I [50] and 3460–3480 cm 1 in cellulose II [47,68,69]) in the IR spectra. There may be between OCH3 at the C-2 position and OH at the C-6 position for 2,3-di-O-MC. There may be between OH at the C-3 position and the adjacent ring oxygen and between OH at the C-2 position and OCH3 at the C-6 position for 6-O-MC. It has been confirmed that such intramolecular hydrogen bonds can be formed in either solid film or homogeneous solution states [69–72]. The formation of such intramolecular hydrogen bonds has also been observed in a DMSO solution state of 23MC using NMR analyses with deuteration [73]. To investigate the intramolecular hydrogen bonds, the film samples were also analyzed by CP/MAS 13C NMR [67]. Fig. 17 shows the CP/MAS spectra of (1)
80
Kondo
2,3-di-O-MC, (2) 6-O-MC, and (3) Tri-O-MC. The introduction of an O-alkyl group promotes strong deshielding of the 13C nucleus of the substituted carbinol group, usually by ca. 9 ppm in solution NMR [74,75]. In the spectra of cellulose ethers, this characteristic should be reflected in the chemical shifts of carbons at C-2, C-3, and C-6 positions bearing alkoxy substituents. Thus peak assignment was carried out in the CP/MAS 13C NMR spectra of the film samples using the solution-state 13C NMR results of Parfondry and Perlin [76]. Unsubstituted C-2, C-3, and C-5, and substituted C-6 carbon signals in 6-O-MC overlapped to some extent with each other in the range of 77–70 ppm. Signals of the C-2, C-3, and C-6 carbons shifted to downfield (ca. 10 ppm) by methyl substitution. In the 2,3-di-O-MC and Tri-O-MC, the C-4 carbon signals, which are assignable in cellulose, shifted upfield by substitution of the adjacent OH groups at the C-3 position and overlapped with the C-5 carbon signal. Signals of C-2 and C-3 carbons in the two MCs overlapped with each other and cannot be identified because of their similar and strong deshielding of 13C nuclei of completely substituted methoxy groups at both positions. Considering a weak deshielding effect of the intramolecular hydrogen bonds between the methoxy oxygen at the C-2 position and the OH groups at the adjacent C-6 position as described later, the C-2 carbon may resonate
Figure 15 IR spectra of film samples of cellulose, 2,3-di-Oand 6-O-substituted cellulose derivatives in the region of OH stretching vibration. MC: O-methylcellulose; EC: O-ethylcellulose; AC: O-allylcellulose; and BC: O-benzylcellulose.
Figure 16 Curve fitting for OH stretching regions in 2,3-diO-MC and 6-O-MC.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
Figure 17
CP/MAS
13
81
C NMR spectra of regioselectively substituted O-methylcelluloses (MCs).
upfield to the C-3 carbon. Only the C-1 signal is easily assignable as it is completely separated from other signals. The presence of an ether substituent at the C-2 position causes an upfield shift of the C-1 resonance relative to that of the glucose residue [76]. Therefore it is assumed that the C-1 resonances may have an upfield shift similarly by the hydrogen bonding formation at the adjacent C-2 position. Naturally, the change in the hydrogen bonding arrangement should be more weakly attributed to the chemical shift of C-1 carbon than the effect due to the substitution of the OH at the C-2 position. Kamide et al. [70] reported that the chemical shift of the C-1 carbon may appear to have an upfield value of more than 105 ppm in the case of the intramolecular hydrogen bond between the C-2 and C-6 positions (Fig. 14A and C). They also mentioned that the C-1 chemical shift may have a field value lower than 105 ppm in the case of the free OH at the C-2 position that did not include the hydrogen bond between the C-2 and C-6 positions. The latter case was based on the assumption that a seven-membered k–jelectron conjugate system is formed in a cellobiose unit [C-4-O-C-1V-O5V-HO-3-C-3-C-4: consider the case without the intramolecular hydrogen bond between C-6 and C-2V in Fig. 14(A)]. In Table 3, the C-1 chemical shifts of 6-O-substituted cellulose derivatives except 6-O-tritylcellulose show smaller values than 105 ppm, suggesting the existence of intramolecular hydrogen bonds between the C-2 and C-6 position. From this result and FT-IR analyses, it is indicated that in the 6-O-substituted cellulose derivatives except 6-O-tritylcellulose, two intramolecular hydrogen bonds (O6-HO-2V and 3-OHO5V) form predominantly and the strengths of the two bonds may be almost equivalent (Fig. 14C). The C-1 chemical shifts of 2,3-di-O-substituted cellulose derivatives in Table 3 also show smaller values than 105 ppm. This indicates the formation of the intramolecular hydrogen bonds between O2-HO-6V (Fig. 14B) in addition to intermolecular hydrogen bonds at the C-6 position. As for tri-O-substituted cellulose ethers, the C-1 signals appeared more upfield than those of 2,3-di-O- and 6-O-substituted cellulose derivatives. Only tri-O-methylcellulose shifted downfield compared with other tri-O-substituted cellulose derivatives. To explain these phenomena, the above explanation of chemical shifts with the hydrogen
bonding formation effects cannot be simply applied to the C-1 signals of the tri-O-substituted derivatives. Because the substitution of both C-2 and the adjacent C-6 hydroxyls can cause a mutual repulsion between the two substituents, the interaction occurring among them can be of different types such as hydrophobic linkage and hence the conformation of the main chain should change. As discussed in the previous section using FT-IR, CP/ MAS 13C NMR may suggest the type of the hydroxymethyl conformations, gt or tg at the C-6 positions in carbohydrates. Horii et al. indicated [6] that the C-6 carbon resonance occurs only as a singlet near 64 ppm in the case of the gt conformation, whereas a resonance band near 66 ppm will appear when the tg conformation is present within the crystalline structures, as shown in Fig. 18 [6]. According to them, the chemical shifts fall into three groups of 60– 62.6, 62.5–64.5, and 65.5–66.5 ppm, which are related to gg, gt, and tg conformations, respectively. In fact, the chemical shift of the C-6 for cellulose II [77–80] indicated the gt conformation, which agrees with the recent result from the neutron fiber diffraction analysis as described above [35]. In the regioselectively methylated cellulose ethers shown in Fig. 17 and other experiments, the chemical shifts of the C-6 were 61.58 and 61.66 ppm for 2,3-di-OMC and 3-O-MC [81], respectively. These results show that the conformation of the OH groups at the C-6 position for the two regioselectively methylated cellulose derivatives
Table 3 Comparison of Chemical Shifts at the C-1 Positions of Anhydroglucose Unit in CP/MAS 13C NMR Spectra of Various Cellulose Derivatives Sample
6-O-
2,3,di-O-
Tri-O-
Methyl cellulose Ethyl cellulose Propyl cellulose Decyl cellulose Allyl cellulose Benzyl cellulose Trityl cellulose
104.1 103.8 102.8 104.2 103.1 103.2 105.5
103.9 103.5 104.5 104.4 103.9 102.4 —
106.5 102.2 102.6 LCa 102.5 102.0 —
a
LC: Liquid crystal at room temperature.
82
Figure 18 13C chemical shifts of the CH2OH carbon vs. torsion angles v around the exo-cyclic C–C bonds. a: a-D-glucose; b: a-D-glucose H2O; c: h-D-glucose; d: h-D-cellobiose; e: a-D-lactose H2O; f: h-lactose; g: sucrose; h: a-melibiose H2O; i: h-methyl cellobioside CH3OH.
Kondo
number, two intramolecular hydrogen bonds expected to be formed in 6-O-MC were maintained in 6-O-alkylcelluloses. Only in 6-O-decylcellulose there appeared a small shoulder around 3600 cm 1. In the case of electron-withdrawing substituents such as allyl and benzyl groups that are easy to form cations (Fig. 15C and D), the hydroxyl frequencies also appeared sharp and symmetric, although there was a slight shoulder at around 3580 cm 1. However, a remarkable shoulder of hydroxyl frequencies appeared at around 3580 cm 1 in both an electron-withdrawing and bulky trityl substituent as shown in Fig. 20. In general, hydroxyl frequencies at 3584–3650 cm 1 are considered as absorption band of ‘‘free’’ OH groups [54,71]. Hydroxyl frequencies due to the intermolecular hydrogen bonds were reported as 3305, 3350, and 3405 cm 1 by Marchessault and Liang [46,47]. The shoulder at 3580 cm 1 in the hydroxyl absorption band of the tritylcellulose was found to be due to rather ‘‘free’’ hydroxyl groups. The OH bands should be broad because of the diversity. Thus an intramolecular hydrogen bond and ‘‘free OH’’ appear to be formed at the C-2 position of the tritylcellulose. The 6-O-tritylcellulose was then multiple-methylated to investigate the behavior of OH groups at the C-2 and C3 positions. The change of distribution of the methyl group as a block of OH groups in a step is monitored in Table 4. As OH groups at the C-2 position were rapidly methylated in the first methylation, the DS of methyl groups at the C-3 position increased slowly in the step. This difference indicates a quick break of hydrogen bond and methylation
may be gg. However, the indication due to the chemical shifts [6] was derived from mono- and oligosaccharides, which have different hydrogen bonding engagements from the present samples. As mentioned already, even hydrogen bonds for celluloses I and II may be totally different from those of 2,3-di-O-MC and 3-O-MC, judging from the OH stretching frequencies in the IR spectra. As the relatively large scattering of data within 2 ppm depending on the conformation at the C-6 may be due to other additional effects such as packing [82] and hydrogen bonding [83,84], the chemical shifts of the C-6 for the regioselectively methylated cellulose derivatives, which are expected to have controlled and specific hydrogen bonds, may not agree with the indication. In addition, the conformation of the glucopyranose ring may be somehow changed by the regioselective substitution by methyl groups. Further studies will be required. 2. Influence of Substituent on the Hydrogen Bonding Formation Hydroxyl frequencies in the IR spectra of 6-O-alkylcelluloses with different lengths of alkyl chains are shown in Fig. 19. The sharp and symmetric shape of the IR spectrum for 6-O-MC did not show a significant change with increasing of alkyl chain length. It suggests that irrespective of the alkyl chain length with the range of 1 to 10 in carbon
Figure 19 IR spectra of 6-O-alkylcellulose films in the region of OH stretching frequencies: (a) 6-O-methylcellulose; (b) 6-O-ethylcellulose; (c) 6-O-propylcellulose; and (d) 6-Odecylcellulose.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
83
Table 4 Degree of Substitution at Individual Positions in 6-O-trityl- and Methylated Tritylcellulose Derivatives
2,3-di-O-methyl-6-O-tritylcellulose prepared in another way [64]. This indicates that ‘‘free’’ OH groups coming from the hydroxyl group at the C-2 position and scission of intramolecular hydrogen bonds at the C-3 position were methylated. CP/MAS 13C NMR spectra of the above samples also showed the same behavior of the hydroxyl groups through methylation (Fig. 21). Broad C-1 signal at 105.5 ppm in the tritylcellulose shifted to upfield peak that has three peak tops at 105.5, 102.5, and 101.4 ppm in MTC1 (Fig. 21 (2)). Each peak top at the three values is due to ‘‘free OH’’, the intramolecular hydrogen bond, and methylation of hydroxyl groups at the C-2 position, respectively. The broad C-1 signal of the tritylcellulose also has a shoulder at around 102.5 ppm due to the intramolecular hydrogen bond. Judging from the C-1 peak shape, the region around 105.5 ppm is main and the vicinity at 102.5 ppm is relatively small. This indicates that the free OH is the one, rather than the OH engaged in the intramolecular hydrogen bonds at the C-2 position. When the methylation proceeded, the peak top at 105.5 ppm decreased as the other two peak tops appeared distinguishably. The peak top at 102.5 ppm decreased and eventually the C-1 signal became one peak at 101.4 ppm in 2,3-di-O-methyl-6-O-tritylcellulose whose OH groups
Sample
X2
X3
X6
6-O-TC MTC1 MTC2 MTC3
0 0.74 0.82 0.84
0 0.55 0.66 0.73
Trityl Trityl Trityl Trityl
Xn: DS on the OH of Cn (n=2, 3, and 6).
of the free hydroxyl groups at the C-2 position, and a slow scission of the intramolecular hydrogen bond between C-3 and O5 through three methylation steps. Namely, the first apparent change in the IR spectrum of methylated tritylcellulose is attributed to the behavior of the hydroxyl group at the C-2 position. In the traces of Fig. 20, as the methylation step preceded, the intensity of the absorption band at 3484 cm 1 decreased gradually and the shoulder at 3580 cm 1 got smaller and sharper. In Fig. 20, the absorbance of the OH bands for the MTCs was normalized on the basis of the internal standard band at 1596 cm 1 due to the trityl group which was not affected by the methylation, and the peak heights between 6-O-TC (tritylcellulose) and MTC1-3 were not comparable with each other. Eventually, OH frequencies mostly disappeared and all hydroxyl groups were almost completely methylated in
Figure 20 Change of OH stretching frequencies in IR spectra of tritylcellulose through the multiple methylation step. 6-O-TC: tritylcellulose; MTC1-3: see Table 4.
Figure 21 Change of the C-1 chemical shift of tritylcellulose and methylated tritylcellulose derivatives: (1) 6-O-tritylcellulose; (2) MTC1*; (3) MTC2*; (4) MTC3*; and (5) 2,3-di-Omethyl-6-O-tritylcellulose. *See Table 4.
84
Kondo
were almost completely blocked by methyl. This phenomenon also indicates that ‘‘free OH’’ at the C-2 position is rapidly methylated and then scission of the intramolecular hydrogen bonds at the C-2 position occurred and finally all hydroxyl groups at the C-2 position were completely methylated. 3. Assignment of ‘‘Free’’ Hydroxyl Groups in Cellulose As described in the above section, Kondo et al. have extensively characterized intra- and intermolecular hydrogen bonds involved in cellulose derivatives using regioselectively methylated cellulose derivatives as model compounds by FT-IR and CP/MAS 13C NMR analyses. It mentioned that not only the assignments due to inter- and intramolecular hydrogen bonds but also the IR interpretation of ‘‘free’’ or non-hydrogen-bonded hydroxyl groups should be of importance to characterize the formation of hydrogen bonds. So far not many papers reported on the IR interpretation of ‘‘free’’ or non-hydrogen-bonded hydroxyl groups. Kondo attempted to assign the ‘‘free’’ hydroxyl groups in the IR absorption bands [68]. In the multiple-methylated derivatives (MTC1V-3V) from 6-O-tritylcellulose (6TC), which have a different distribution pattern from the above MTC1-3, the methyl substitution behavior of hydroxyl groups at the C-2 and C-3 positions in 6TC was monitored by FT-IR (Fig. 22) together with the change of the DS of methyl and the remaining hydroxyl groups at each position for the above four samples determined by gas-chromatographic analyses for the hydrozates of the polymer (Table 5). All spectra in Fig. 22 were normalized on the basis of the internal standard band at 1596 cm 1 due to trityl groups that are not affected by the methylation. In the C–H stretching regions from 2800 to 3100 cm 1, the methylation had an influence obviously on each spectrum. Even in the 23M6TC spectrum shown at the bottom of Fig. 22, the hydroxyl absorption band was slightly observed. This band cannot be noise because S/N ratio in this FT-IR machine was better than 1/15,000. The same band shape was also observed carefully in the other tri-O-substituted derivatives that were already prepared in previous papers [65,67].
Figure 22 Change of IR spectrum for the methylated 6-Otritylcellulose (MTC1V–3V) and 2,3-di-O-methyl-6-O-tritylcellulose (23M6TC) prepared from 6-O-tritylcellulose (6TC).
Considering that the product was very similar to these tri-O-substituted derivatives and that the remaining OH groups were quite small, the IR absorption bands cannot be considered simply due to hydrogen-bonded OH groups; they may be due to ‘‘free’’ or non-hydrogen-bonded hydroxyl groups. In other words, a trace amount of hydroxyl groups in the original tritylcellulose remained intact during this methylation process, possibly because of heterogeneity in the reaction mixtures. Thus when the film sample for FT-IR measurements was cast from the clear solution of
Table 5 Distribution of Methyl and Hydroxyl Groups in Regioselectively Methylated 6-O-tritylcellulose Derivatives
Sample MTC1V MTC2V MTC3V 23M6TC
DS at positions
DS of OH at each position
Overall DS
X2
X3
X6
OH-2
OH-3
OH-6
1.39 1.67 1.68 1.80
0.82 0.91 0.91 0.92
0.57 0.76 0.77 0.88
— — — —
0.18 0.09 0.09 0.08
0.43 0.24 0.23 0.12
Xtri Xtri Xtri Xtri
Overall DS equals X2+X3+X6. Each Xn was determined by a gas chromatographic analysis. Xn is the mole fraction of glucitol derivatives substituted on the OH of Cn (n=2, 3, and 6). DS of OH-n = 1-Xn; Xtri: degree of trityl substitution.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
85
Figure 23 Curve fitting and peak assignments for OH stretching regions in 23M6TC.
the product powder, the molecules in the powder may have rearranged to give ‘‘free’’ hydroxyl groups in the film. The probability of the formation of intermolecular hydrogen bonds in this film is fairly low because neighboring hydroxyl groups are rare; the intramolecular hydrogen bonds can occur: between OH at the C-3 position and the adjacent ring oxygen, between OCH3 at the C-2 and OH at the C-6 positions, and between OH at the C-2 position and OCH3 at the C-6 position. As reported by Kondo [18], the intramolecular bonds may still be maintained even in the homogeneous solution state. The formation of such intramolecular hydrogen bonds has also been observed in a DMSO solution state of 2,3-di-O-methylcellulose (23MC) using NMR analyses with deuteration [81]. To assign the IR band due to free OH groups, it is necessary to evaluate the contribution of the intramolecularly hydrogen-bonded OH groups. In addition, the three hydroxyl groups at each position are quite different in the sense that secondary hydroxyl groups at the C-2 position are influenced by the anomeric C-1 carbon, secondary hydroxyl groups at the C3 position are favorable to form the intramolecular hydrogen bonds, and the hydroxyl groups at the C-6 position are primary OH. Therefore the hydroxyl groups at each position can exhibit three different IR absorption bands. The IR absorption bands for OH stretching regions in 23M6TC of Fig. 22 were deconvoluted into three bands for the curve fitting as shown in Fig. 23. To improve the calculation, the peaks needed to be well resolved, and the number of peaks, the positions, and the areas were accurately determined. Three was employed as the number of peaks and the position was determined by the point at which the second derivative of the spectrum contained peaks. All other parameters in the calculations were vari-
able. After the best curve fitting, the peak positions of the three deconvoluted bands were 3579, 3558, and 3489 cm 1, respectively. The two bands (3579 and 3558 cm 1) were assigned to the free hydroxyl groups because they appeared at higher wavenumbers than those for inter- or intramolecular hydrogen-bonded hydroxyl groups in cellulose (Tables 1 and 2). As a reference for the IR band due to free hydroxyl groups, it is reported that the free OH in secondary alcohol appears at 3620–3635 cm 1, whereas the free OH for primary alcohol shows bands at 3630–3645 cm 1 [85]. The difference in the band positions between cellulose and alcohol can be due to the regiochemical effects in cellulose.
Table 6 The Results from a Curve Fitting Method Applied to the Methylated Tritylcelluloses, MTC1–MTC3 and 23M6TC. Each Correlation Coefficiency (R2) is Better than 0.99 Three peaktops of the deconvulated IR bands
MTC1V MTC2V MTC3V 23M6TC
a (cm 1)
b (cm 1)
c (cm 1)
3579 3577 3578 3579
3513 3552 3559 3558
3480 3486 3487 3489
OH2
OH-6
Intramolecular H-Bonds
86
To assign the three OH bands, the corresponding deconvoluted IR bands in partially methylated tritylcelluloses as cast films, MTC1V–MTC3V, were compared with those for 23M6TC. The results are shown in Table 6. IR absorption bands in the OH stretching region for each sample were also deconvoluted into three IR bands (a, b, and c in Fig. 23) with peak tops at around 3580, 3555 (‘‘free’’ hydroxyl groups), and 3485 cm 1, respectively. The wave number of band c with a lower peak top at 3485 cm 1 coincides with that calculated for intramolecular hydrogen-bonded hydroxyl groups in regenerated cellulose (Table 2) and is very close to the assignment (3470–3480 cm 1) proposed for intramolecular hydrogen-bonded hydroxyls using regioselectively methylated cellulose derivatives in Fig. 15 [17] and Fig. 14B and C, between OH at the C-3 position and the adjacent ring oxygen, between OCH3 at the C-2 position and OH at the C-6 position, and between OH at the C-2 position and OCH3 at the C-6 position. Considering these results, band c in Fig. 23 may involve not only the intramolecular hydrogen bonds at the C-3 position, but also possible intramolecular hydrogen bonds between the functional groups at the C-2 and C-6 positions. Therefore some of the free hydroxyl groups at the C-2 and C-6 positions may contribute to band c, which may be the reason for the inconsistency between FT-IR results and OH values determined by the gas chromatographic method as shown in Table 5. Bands a and b, because of the remaining free OH groups at either C-2 or C-6 position which were not tritylated in 6TC (although some of them may contribute to intramolecular hydrogen bonds), can be assigned in the following way: The original IR bands in Fig. 23 show two peak tops at 3575 and 3485 cm 1, where bands a and c are mainly indicated, and their relative intensities change depending on the samples (MTC1V-3V in Fig. 22). In contrast, the relative intensity of band b does not change significantly. During this multiple methylation process, the OH groups at the C-2 and C-3 positions are replaced and their FT-IR spectra are affected. On the other hand, for the OH at the C-6 position, which was a trace amount from the beginning, the influences are small. Thus bands a and b with peak tops of 3580 and 3555 cm 1 are assigned to free OH at the C-2 and C-6 positions, respectively. Furthermore, the two peak positions of bands a and c did not shift significantly from 23M6TC to MTC1V as shown in Table 6. However, the peak position of band b at 3558 cm 1 changed to a lower wave number between MTC2V (3552 cm 1) and MTC1V (3513 cm 1). This indicates that intramolecular hydrogen bonding at the C-6 position starts to perturb the OH bands.
Kondo
molecular association can be categorized in cellulose. A major consideration is that the predominant crystalline state of cellulose is included as a component in the ordered state. This means that the ordered state also contains noncrystalline-ordered states. The category ‘‘ordered’’ is in contrast to the ‘‘nonordered’’ state which, to date, has been considered as ‘‘amorphous cellulose’’ for lack of a useful way to characterize the product. It should be noted that the amorphous state being categorized as the ‘‘nonordered’’ state should be distinguished from the ‘‘noncrystalline state of cellulose. Thus in this classification it becomes crucial whether the state is ‘‘ordered’’ or ‘‘nonordered.’’ The relationship is schematically illustrated in Fig. 24 [5]. Historically, it has been difficult to find an appropriate method to characterize noncrystalline or amorphous domains of cellulose. Often, wide-angle X-ray diffraction (WAXD) has been used for determining the crystalline forms and the crystallinity; however, in most cases when WAXD provides a diffuse diffraction pattern, it is considered simply as ‘‘amorphous cellulose.’’ However, as mentioned above, noncrystalline state does not necessarily indicate amorphous state. Noncrystalline state includes both liquid crystalline and nematic-ordered cellulose [5] that exhibits a certain order state, whereas amorphous state does not own any preferred orientation. Thus we have attempted to determine the ‘‘noncrystalline regions’’ of noncrystalline cellulose films using FT-IR monitoring of the deuterated hydroxyl groups [86]. We have found that such noncrystalline regions may comprise at least three different domains. The study [86] also indicated the presence of ordered domains in the noncrystalline regions. As the regioselectively methylated celluloses, 23MC (64), 6MC(66), and tri-O-methylcellulose (236MC)(65) had a controlled distribution of substituents and thus hydrogen bonds, they were considered to be model compounds for amorphous cellulose and hence ideal in examining the relationship between polymer structure and the
C. Hydrogen Bonds in Noncrystalline or Amorphous Cellulose 1. Noncrystalline Cellulose and Amorphous Cellulose Cellulose, which is a h-1,4-linked glucan homopolymer, is normally classified according to how the h-glucan chains associate. We expand the concept of how various states of
Figure 24
Concept of glucan chain association for cellulose.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
physical properties of cellulose and its derivatives in terms of hydrogen bond formation. It is noted that pure cellulose tends to order somehow in a certain way, so that it is difficult to keep amorphous state in cellulose if it can be obtained. In the previous sections, FT-IR spectroscopy was used to identify intra- and intermolecular hydrogen bonds in the regioselectively synthesized 23MC and 6MC. Films of 23MC and 6MC exhibited narrow OH stretching bands in their IR spectra because of the controlled hydrogen bonding (Fig. 13). Morphologically, films cast from these methylcellulose derivatives were also found to be predominantly noncrystalline or rather amorphous than crystalline. Therefore the narrow OH absorbance bands and the amorphous homogeneity of the sample microstructure enabled us to clarify and classify the interchain hydrogen bond interactions found in the samples. It is believed that a characterization of the hydrogen bonds found in amorphous cellulose would be of fundamental value and, furthermore, that a structural study of amorphous cellulose in light of hydrogen bonding might be a first step in uncovering details of how molecules rearrange in going from the liquid to the crystalline state. So-called ‘‘amorphous cellulose’’ samples are usually prepared by ball milling of cellulose [87,88] by deacetylation of cellulose acetate with sodium methoxide in anhydrous methanol [89], or by precipitation from nonaqueous solvent systems into nonaqueous regeneration media with the avoidance of stress [90–94]. To date, most of these samples have been studied by WAXD [87–95], FT-IR spectroscopy [95], and solid-state NMR [94]. Hatakeyama and Hatakeyama [96] have previously reported on the formation of interchain hydrogen bonds with increasing temperature for amorphous regions in cellulose fibers. More recently, Kondo and Sawatari [24] have tried to analyze and comment on the types of hydrogen bonds formed in amorphous cellulose. The methodology was threefold: (1) to quantitatively produce an artificial IR spectrum for amorphous cellulose by using a combination of amorphous methylcellulose model compound IR spectra; (2) to characterize the difference between the real and the artificial spectra in terms of the formation of hydrogen bonds; and, finally, (3) to compare the result of (2) with the IR spectra of propyl alcohol solutions, which can serve as model systems for intermolecular hydrogen bonding. This approach lets us draw a number of conclusions about the hydrogen bonds formed at the C-2 and C-3 positions in the anhydroglucose repeating units of amorphous cellulose. For this investigation, all film materials (cellulose, 23MC, 6MC) used should have a nonordered amorphous microstructure at the level of WAXD patterns as shown in Fig. 25. Fig. 13 shows the OH frequency region of the IR spectra for each amorphous homopolymer film sample investigated. By using these four spectra and by quantitative manipulation, the artificial spectrum could be constructed as illustrated in Figs. 26b and 27b. The IR spectrometer software produced a list of the most prominent bands in this artificial IR spectrum in the region being
87
Figure 25 Wide-angle X-ray diffraction patterns for cast films: (A) cellulose, (B) 23MC, (C) 6MC, and (D) a blend of 23MC and 6MC (1.08/1 w/w).
studied, and Table 7 shows the most probable assignment for these bands, as well as those found in a real amorphous cellulose sample. Figs. 26 and 27, respectively, show OH and C–O stretching vibration regions resulting from the glucose ring skeletal vibration. In comparing the real and the artificial spectra for the amorphous cellulose, there is no significant difference in the ring stretching vibration region as clearly illustrated in Fig. 27. This indicates that any absorption contributions by methyl groups may be precluded in the methylated samples to the ring stretching vibrations. Thus the artificial spectrum mirrors the glucose ring structure found in real amorphous cellulose. The data contained in Table 7, which lists typical absorption frequencies for the two spectra, also seem to support this hypothesis. In regard to the stretching and bending vibrations for methine and methylene groups in cellulose, the quantitative mathematical model could not completely remove the contribution by methyl groups in the methylated samples to totally match the artificial spectrum for amorphous cellulose. Difference Between the Real and the Artificial Spectra There is a marked difference in the OH stretching region of the real and the artificial IR spectra. The difference spectrum (real artificial; Fig. 26a–b) is shown in Fig. 28 with the region between 3750 and 3000 cm 1 expanded to clearly show this marked difference. Considering that the artificial spectrum was constructed assuming a linear contribution by the intra- and intermolecular hydrogen bonds at the C-6 position, the difference spectrum should thus contain peaks arising from intermolecular hydrogen bonds at the C-2 and C-3 positions and any ‘‘free’’ hydroxyl groups. Of course, the bands resulting from common hydrogen bonds in both the real and the artificial
88
Kondo
Figure 26 IR spectra in the OH stretching vibration (3750–3000 cm 1) region: (a) real spectrum of amorphous cellulose film, (b) artificial spectrum, and (c) spectrum for the blend sample (23MC/6MC=1.08/1 w/w).
spectra are not completely canceled out by subtraction because in the two spectra the magnitude for each OH absorbance band is not necessarily of equal value. The difference spectrum can thus include, to a greater or lesser extent, all the hydrogen bonds present in pure amorphous cellulose. However, the marked differences in the two spectra cannot adequately be explained simply in terms of unequal contributions from common hydrogen bonds: the two positive peaks and negative valley in the difference spectrum are attributed to intermolecular hydrogen bonds at the C-2 and C-3 positions as well as ‘‘free’’ OH groups. The main negative and positive peaks in Fig. 28 appeared at two particular wavenumbers, 3472 and 3352 cm 1. Unbonded or ‘‘free’’ OH groups absorb infrared
Figure 27 IR spectra in the C–O stretching vibration (1500– 700 cm 1) region: (a) real cellulose spectrum and (b) artificial cellulose spectrum.
light at 3558 and 3580 cm 1 described in a previous section (see Assignment of ‘‘Free’’ Hyroxyl Groups in Cellulose under Section B) [68], which is a higher wave number than the two peaks. A shoulder around 3580 cm 1 with an absorption of 0.06 may be due to the ‘‘free OH.’’ As all the OH groups in 23MC and 6MC are engaged in some form of
Table 7 Comparison of Typical Absorption Frequencies Between the Real and the Synthesized IR Spectra of Amorphous Cellulose Frequency (cm 1) Synthesizedc
Relative intensitya
669
671
W
899
892
M
1040 1070
1040 1075
S S
1108
1108
S
1159
1154
S
1374 1420
1375 1425
M W
2892 3420
2903 3457
M S
Realb
a
Interpretation OH out-of-phase bending Antisymmetric out-of-phase ring stretching C–O stretching Skeletal vibrations involving C–O stretching Antisymmetric in-phase ring stretching Antisymmetric bridge C–O–C stretching CH bending CH2 symmetric bending CH stretching OH stretching
Key: S, strong; M, medium; W, weak. Real spectrum of amorphous cellulose film prepared by casting. c Synthesized spectrum of amorphous cellulose. b
Hydrogen Bonds in Cellulose and Cellulose Derivatives
89
Figure 28 Difference IR spectrum obtained by subtracting the artificial (Fig. 26b) from the real (Fig. 26a) cellulose spectrum.
hydrogen bonding, the artificial spectrum formed by combining the two contributing spectra is thought to have few ‘‘free’’ OH groups. Therefore the almost negligible signal at 3580 cm 1 in the difference spectrum indicates that there are very few ‘‘free’’ OH groups in the amorphous cellulose itself. A negative absorbance valley at 3472 cm 1 (assigned to intramolecular hydrogen bonds) indicates that the signal was overcanceled in the artificial spectrum, whereas the positive band around 3352 cm 1 was attributed to the intermolecular hydrogen bonding at the C-2, C-3, or C-6 position. The negative valley (3472 cm 1) in the difference spectrum appeared to reflect an excess of the intramolecular hydrogen bonds either at the C-2 position and the OCH3 at the C-6 position, or at the C-6 position and the OCH3 at the C-2 position, or at the C-3 position and the ring oxygen in the artificial spectrum. Interestingly, as the solvent is changed for the same 23MC sample, the crystallinity of the film varies from solvent to solvent and the OH groups at the C-6 position may be favorably involved in an intermolecular hydrogen bonding. The extent of crystallization may be dependent upon the behavior of the primary OH group located at the C-6 position. Stated differently, the OH group at the C-6 position may be significant in determining the final morphological make-up of cellulose. This indicates that when the C-6 hydroxyls in cellulose are, to a great extent, engaged in the intermolecular hydrogen bonding, the resulting cellulose should exhibit high crystallinity. Invoking this hypothesis, either a random distribution of microcrystallites or a series of domains arising from intermolecular hydrogen bonds will result in a highly amorphous state for cellulose. To confirm the existence of these postulated microcrystallites, small angle X-ray scanning (SAXS) intensity distributions were measured using a PSPC system. The SAXS pattern for the amorphous cellulose showed no significant scattering maxima, indicating that there was no lamella structure present in the cellulose. Thus SAXS
and WAXD patterns for the amorphous cellulose gave no support to the idea that microcrystallites were present. It is therefore concluded that the amorphous cellulose must include, to some degree, domains formed by the intermolecular hydrogen bonds at the C-2, C-3, and C-6 positions. Kondo and Sawatari therefore proposed a model for amorphous cellulose in which some amorphous domains are partly interacted by intermolecular hydrogen bonds as illustrated in Fig. 29. This is similar to a fringed micellar structure. In a dilute and semidilute cellulosic solutions Buchard et al. proposed the formation of the fringed micelle to explain the rheological behavior of the cellulosics as shown in Fig. 30 [97–100]. Considering the above results, there may be correlation on the aggregation states between the solution states and amorphous states of cellulose. In other words, from a dilute solution state and a concentrated lyotropic liquid crystalline state to an amorphous and a crystalline solid state there might be a connection in terms of rearrangements through inter and intramolecular hydrogen bonding formation. 2. Hydrogen-Bonded Domain in Amorphous Cellulose Currently, there is a shortage of structural information about the noncrystalline regions including amorphous state, perhaps partly because terminology suggests and impression persists that molecular chains in these regions are completely without structure and partly because methodology has been limited to WAXD and CP-MAS 13C NMR for measuring order in the presence of substantial amount of disorder. It is not uncommon for substrates that are not identifiable as crystalline by a method such as X-ray diffraction to be labeled ‘‘amorphous’’, but the definition of amorphous goes beyond noncrystalline to unorganized and having no pattern of structure as described above [5,101]. Therefore in this section details of the noncrystalline regions are particularly examined in the noncrystalline
90
Kondo
Figure 29
Schematic model for amorphous cellulose.
cellulose film samples, regioselectively methylated 23MC and 6MC amorphous film samples used above, as model components of amorphous cellulose using FT-IR methods [86]. Applications of deuteration methods to IR have so far focused on the separation of IR spectra for cellulose structure into two parts of crystalline and noncrystalline regions, respectively, and then only the discriminated crystalline regions have been studied [44,102,103]. Here,
Figure 30 Schematic drawing to demonstrate various size of particles visualized by changing the angular dependence of light scattering: qRg<<1 (whole particle seen); qRg > 1 (substructures approved). (From Ref. [99]; Courtesy of Prof. Burchard; Hermann Schtaudinger Institute, Freiburg, Germany.)
only the noncrystalline regions in the cellulose model compounds are focused using the FT-IR monitoring of the deuteration process. The main advantage of this method is that the use of a reaction cell has enabled us to obtain not only a change in reproducible and correct IR spectra for noncrystalline regions in cellulose, but also the rate constant for the deuteration reaction which is assumed to correspond to the nature of amorphous regions [86]. Thus it is possible to characterize the morphology of noncrystalline regions by analyzing the diffusion behavior of D2O as a probe. As already described in a previous section, each polymer, 23MC and 6MC, is considered to have different types of inter- and intramolecular hydrogen bonds. Before analyses, it was confirmed that the morphology (smooth or rough) on the surface of the film does not affect the rate constant by comparison of the surface observation by atomic force microscopy (AFM) with the rate constants for differently prepared two film samples with different morphologies on the surfaces. Fig. 31 shows the change in IR spectra for 6MC accompanied by the deuteration process. When the deuteration proceeded, OH stretching vibration around 3470 cm 1 decreased, and instead the bands at 2559 cm 1 due to OD at the C-2 and C-3 positions appeared and then increased. Similar behaviors were observed for the OH and OD bands in the amorphous 23MC and cellulose. However, the deuteration was not completed regardless of the amorphous samples, giving intact OH groups. The amount of the unexchangeable OH was 14.3%, 10%, and 13.3% for 6MC, 23MC, and noncrystalline (amorphous) cellulose, respectively. These unexchangeable hydroxyl bands may also indicate the presence of domains involving the intermolecular hydrogen bonds in a proposed amorphous model of Fig. 29 [24]. Here the OH–OD exchange reaction can be postulated to obey pseudo-first-order kinetics because of the large amount of D2O to the amount of OH in each film sam-
Figure 31 Changes of OH and OD in IR absorption bands for monitoring the deuteration of amorphous 6MC.
Hydrogen Bonds in Cellulose and Cellulose Derivatives
ple. The general equation, d[OH]/dt=k[OH], can be employed. Thus the derived relationship, ln{[OH]t /[OH]0 }= kt, was drawn in Fig. 32 for the three amorphous samples, 23MC, 6MC, and cellulose, respectively. Each of the three samples showed similar kinetic behaviors that were divided by three single reactions. In other words, three kinds of exchange reaction (1, 2, and 3 in Fig. 32) can competitively coexist. Table 8 shows the rate constants for each reaction. The rate constant for reaction 1 was rela-
91 Table 8 Rate Constants (k) from OH to OD for Every Single Reaction in the Deuteration Processes of the Amorphous Three Film Samples Time course (hr)
k (hr 1)
R2
0.08–5 0.08–4 0.08–2
0.136 0.247 0.264
0.98 0.99 1.00
6–12 5–13 3–12
0.085 0.057 0.075
0.98 0.99 0.98
Reaction 1 23MC 6 MC Cellulose Reaction 2 23 MC 6 MC Cellulose R: Correlation coefficient.
tively different among the three samples. On the contrary, the rate constant for two reactions seems to be similar among them. Of course, this is still speculative. In general, adsorption and diffusion in crystalline polymers are considered to occur in noncrystalline or amorphous regions. However, it is very complex because the structure for the crystalline regions may somehow have influences on it although the morphological effects on the surface have no influence. Considering that the samples exhibited noncrystalline for the X-ray measurements, noncrystalline regions in these cellulosics may be discriminated into three phases: (1) deuteration is fast, corresponding to reaction 1; (2) deuteration is slower, corresponding to reaction 2; and (3) almost undeuterated, corresponding to reaction 3. Interestingly, the second rate constants among the three samples were very similar although the first rate constants for them differed. This indicates that the second one may correlate with the deuteration for the intramolecular hydrogen bonds (Fig. 6) in noncrystalline or amorphous phases which are common interactions among the above three samples. Further investigation will be needed because the type of intermolecular hydrogen bonds found at the C-2, C3, and C-6 hydroxyl positions participates, to some extent, in determining the structure of amorphous cellulose [25].
D. The Relationship Between Intramolecular Hydrogen Bonds and Certain Physical Properties of Regioselectively Substituted Cellulose Derivatives
Figure 32 The relationships between decreasing ratio of OH groups, ln{[OH]t/[OH]0} and time, t, during the deuteration process for the three amorphous samples, 23MC, 6MC, and pure cellulose.
To date, the author has focused on clarifying the hydrogen bonding formation involved in cellulose molecules in various states, such as blends, gels, amorphous, and liquid crystals [17–28,67,68,104], by using regioselectively substituted methylcelluloses such as 23MC(64) and 6MC(66) as cellulose model compounds. These investigations were performed mainly by using tools such as FT-IR, DSC, fluorescence spectroscopy, and solid-state NMR. Interestingly, the OH absorption band in the IR spectrum of 6MC films was sharper and more symmetric than those for
92
23MC, which has only one OH group per anhydroglucose unit. This phenomenon was also observed for other substituents with longer alkyl, benzyl, and allyl groups. To clarify this behavior, a model was proposed to explain the formation of intramolecular hydrogen bonds in 6-O-substituted cellulose derivatives. Specifically, these cellulose derivatives have two intramolecular hydrogen bonds, one between the OH at the C-3 position and an adjacent ether oxygen of the glucose ring, and the second between the ether oxygen at the substituted C-6 position and an adjacent OH at the C-2 position (Fig. 14). Accordingly, the aggregation state of 6-O-substituted compounds should be interesting to study particularly in terms of any relationship between the formation of the hydrogen bonds and their direct effect on certain physical properties. In general, the formation of inter- and intramolecular hydrogen bonds in cellulose and its derivatives is considered to have a strong influence on their physical properties. However, only a few published reports [48,105,106] have dealt directly with the above point of view, although many papers [107, 108] have referred indirectly to this relationship between structure and physical properties. Therefore one 6-O-substituted cellulose ether, namely, 6-O-methylcellulose, which has been revealed to have mainly intramolecular hydrogen bonds, was chosen and its physical properties including solubility, hydroxyl reactivity, and crystallinity, which should be influenced directly by any intramolecular hydrogen bonds, were investigated as follows [19]. Three typical properties chosen to study were the solubility, the relative reactivity of the remaining OH groups at the C-2 and C-3 positions in a repeating unit, and the crystallinity in order to answer the following four questions: (1) Can the polymer be easily dissolved in various solvents due to a lack of intermolecular hydrogen bonds? (2) Is it possible to maintain intramolecular hydrogen bonds after dissolution to allow the solution to have an influence on the OH reactivity mentioned above? and (3) Is the solution less likely to crystallize than other ordinary cellulose and cellulose derivatives because of a restriction in the intermolecular hydrogen bonding which is available to the crystallizing polymer? (4) Is there any influence of intramolecular hydrogen bonds on the determination of the handedness of cholesteric twist sense of ethylcellulose lyotropic mesophases? Solubility Table 9 lists the solubility of methylcelluloses, 23MC, 6MC, and three kinds of methylcelluloses normally prepared commercially in an aqueous system so as to have different DS. In general, for cellulose derivatives, the higher the DS the higher the solubility of the derivative to organic solvents. However, interestingly enough, 6MC having a lower DS showed a higher solubility than did 23MC with a DS of 2.0. As shown in a previously published paper [67,68] the FT-IR spectra for 23MC and 6MC showed this was due to the presence of interchain hydrogen bonds at the C-6 position of 23MC. Further, in comparing both 23MC with a DS of 2.0 and 6MC with
Kondo Table 9 Solubility of Various Methylcellulose (MC) Commercial MC Solvent Water Aq. alkali (pH 9.5) Aq. acid (pH 5.5) Acetone Methanol THF Chloroform DMSO DMAc
DS 0.1–1.1
DS 1.4–2.0
DS 2.4–2.8
23MC DS 2.0
6MC DS 1.0
D o
o D
D
D
o
o
D
o
oD
oD oD
o o
o o oD oD
D D o o
o o o o o o
o: Soluble; D: swelling; : insoluble; oD: partially soluble.
a DS of 1.0 with other methylcelluloses having a corresponding DS, respectively, the solubility of both 23MC and 6MC exhibited remarkable differences. In particular, 6MC, which has mainly intramolecular rather than intermolecular hydrogen bonds, exhibited more favorable solubility in solvents having different polarities. These results indicated that the solubility of 6MC is mostly determined by the absence of interchain hydrogen bonds that can obstruct swelling and solvation of the polymer. Primary OH at the C-6 position can favorably form intermolecular hydrogen bonds [18–20,23,24], causing poor solubility of the material to solvents. In other words, the amount of free OH groups at the C-6 position may contribute more critically to determining the solubility of the material than that of free OH groups at the C-2 or C-3 position. In fact, comparing 6MC with MC of DS 2.4–2.8 in Table 9, primary OH-6 was fully substituted for 6MC whereas for the MC with DS 2.4–2.8 unsubstituted OH-6 was more or less remaining. Therefore it may cause the superior solubility for 6MC to the MC with 2.4–2.8 although total DS for the latter MC is higher. Relative Reactivities of the Remaining OH Groups at the C-2 and C-3 Positions Concerning the difference in relative reactivity of the hydroxyl groups (OH-2, OH-3, and OH-6, respectively) at the two (C-2), three (C-3), and six (C-6) positions of the anhydroglucose unit, it is well known [109,110] that the order of the relative reactivity is OH-2>OH-6>OH-3 for MC prepared from alkali-cellulose in an aqueous solvent system. The higher reactivity of OH-2 has been postulated to be due to its high acidity that is enhanced by its proximity to the anomeric center, C-1 [111]. Therefore, if an intramolecular hydrogen bond was still present at the C-2 position even in the reaction mixture, then the reactivity of OH-2 should be altered, and it would probably be reduced. Within this definition, the relative reactivity of the remaining hydroxyl groups (OH-2 and OH-3) in 6MC,
Hydrogen Bonds in Cellulose and Cellulose Derivatives
6TC, and 6BC was examined. As reported previously [67], the two kinds of 6-substituted derivatives, 6TC and 6BC, are assumed not to have any intramolecular hydrogen bonds; only 6MC has them. From the change in the DS values at the C-2 and C-3 positions before and after the reaction, the relative reactivity was found to be in the following order: 6TC> 6BC>6MC. This is apparently due to the difference in reactivity at the C-2 position. Moreover, this difference is directly attributed to the presence of intramolecular hydrogen bonds at the C-2 position. As described in a previous section, the introduction of electron-withdrawing and bulky functionalities such as trityl and benzyl groups at the C-6 position changes the structure of the intramolecular hydrogen bonds to give free OH groups at the C-2 position and, in addition, the substituent effect of the more bulky trityl group shows itself more in the appearance of free OH-2 than in the smaller benzyl group [67]. Further, the bulkiness of the trityl groups at the C-6 position for 6TC may change the conformation of the glucose backbone to cause, to some extent, a break of the intramolecular hydrogen bonds between the OH at the C-3 position and its neighboring ring oxygen (O-5). Thus, this produced free OH-3 for 6TC which can be more methylated than 6BC. In the case of 6MC, this deformation of the intramolecular hydrogen bonds is not expected by the substitution at the C-6 position. Therefore the order of 6TC>6BC>6MC above can be considered as the reverse order of preference for the formation of intramolecular hydrogen bonds. Indeed, in 6MC that has strong intramolecular hydrogen bonds, the relative reactivity at both the C-2 and C-3 positions exhibited almost the same values, which was distinctly different for both 6TC and 6BC. This does not mean an enhanced reactivity of the OH-3 reactivity, but rather a reduction in the OH-2 reactivity probably due to the formation of intramolecular hydrogen bonds at this position. Simultaneously, the hydrogen bonds at the C-2 position which form between OH-2 and the ether oxygen of a methoxy group at the C-6 position seem to be very similar to the intramolecular hydrogen bonds at the C-3 position, between OH-3 and the glucose ring oxygen. Therefore reactivity at both the C-2 and C-3 positions shows similar values. In contrast, 6TC and 6BC exhibited relative reactivity in the order of OH-2>OH-3. Taking hydrogen bonding into account, this order is reasonable and coincides with that usually exhibited in aqueous systems as mentioned previously. In this study, it is noted that the methylation was performed in homogeneous DMSO solution, and therefore the hydroxyl groups in 6TC and 6BC may be solvated to prevent further involvement of the hydrogen bonds. In 6MC, as stated above, the relative reactivity at the C-2 and C-3 positions indicates that the intramolecular bonds were still maintained even in the homogeneous solution state [19,26]. Crystallinity The X-ray diffraction patterns for 6MC films cast from both DMAc and CHCl3/CH3OH(4/1 v/v) solvents
93
exhibited noncrystalline (amorphous) patterns similar to those obtained from noncrystalline celluloses obtained from the DMAc-LiCl and SO2-diethyl amine-DMSO solutions, and further the 6MC did not show a crystalline pattern even after heat treatment at 160jC. Thus 6MC shows poor crystallinity irrespective of the homogeneity of the structural unit along a molecular chain. In general, crystallization depends not only on the regularity of chemical structure but also on sufficient chain flexibility for coordinated molecular motion to form nuclei. The 6MC chain may be sufficiently stiff to form a high viscosity medium during evaporation of the solvent that would prevent nucleation. Therefore precipitation/crystallization in a dilute solution was tried. However, crystallized 6MC could not be obtained after this process. On the other hand, 23MC showed different patterns depending on the solvents. As indicated in previous papers on crystallization [25] and gel formation [20,26] of cellulosics, the primary OH groups at the C-6 position may be favorably involved in interchain hydrogen bonding. The extent of crystallization may depend on the behavior of the primary OH groups. Thus cellulose derivatives whose OH groups at the C-6 position are blocked like in 6MC may prevent crystallization in the same manner as crystallization resulting from interchain hydrogen bonding in, say, 23MC. Stated differently, 6MC, which shows strong intramolecular hydrogen bonds, can perhaps possibly form a crystalline state simply from van der Waals’ force by a minimization of the system potential energy. However, the poor crystallinity exhibited by 6MC described above suggests that interchain hydrogen bonds at the OH groups of the C-6 position may be more advantageous in aiding crystallization in cellulosics than van der Waals’ force. The fact that the uniform structure of 6MC in which every structural unit is completely and regioselectively substituted can engage in intramolecular hydrogen bonds is not an advantage for crystallization, which differs from other synthetic polymers such as polyolefins and polyesters. This might be due to an induced stiffness in the main chain of 6MC, which results from the presence of intramolecular hydrogen bonds. Concerning precedence for the primary OH at the C6 position to the secondary OH at the C-2 and C-3 positions in crystallization, one reason is that, as described above, 23MC, which has only free primary OH at the C-6 position, was easier to be crystallized than 6MC and yet the crystallized 23MC did not show a melting point. This appears probably due to the strong hydrogen bonding engagements in the crystallized 23MC. As for the favorableness of the interaction, Kondo et al. have already reported [18,23] that in the comparison of 23MC with 6MC for the blend with poly(ethylene oxide) (PEO) which has oxygen in the polymer backbone, only primary OH at the C-6 position for 23MC was engaged in intermolecular hydrogen bonds, whereas secondary OH at the C-2 or C-3 position for 6MC did not form the interaction with PEO. Therefore it is considered that the primary 6-OH may contribute to the crystallization more than the secondary hydroxyls.
94
The Influence of Intramolecular Hydrogen Bonds on Handedness in Ethylcellulose/CH2CL2 Liquid Crystalline Mesophases In 6MC samples there was a direct correlation between the physical properties observed and the formation of intramolecular hydrogen bonds that can even be maintained in solution [19,27]. The intramolecular hydrogen bonds were also found to have an influence on the enzymatic hydrolysis of 6MC [21,22]. Kondo and Gray [64] succeeded in preparing a series of methyl- and ethyl celluloses having a systematically controlled distribution of substituents and DS. These polymers would appear to form an ideal set of complete samples for determining what type of correlation exists between the physical properties and the distribution of substituents for alkylcellulose derivatives in terms of hydrogen bond formation. Thus the effect of substituent distribution on the liquid crystalline properties of EC is the focus in this section. The majority of cellulosic mesophases that have been studied to date are right-handed cholesteric, but a few left-handed systems have also been reported [112–116]. Specifically, lyotropic ethylcellulose (EC) mesophases were observed to show both types of handedness depending on the polymer volume fraction and solvent [112]. Guo and Gray [115,116] reported that cholesteric liquid crystalline solutions of acetylated EC in chloroform exhibited a change in handedness from a lefthanded to a right-handed helicoidal supermolecular arrangement with an increasing acetyl content in the EC. The twist sense of EC mesophases in chloroform and CH2Cl2 was also observed to change from left-handed to righthanded with an increasing degree of ethyl-substitution in EC [117]. However, the driving force for this structural reversal is still not clear. Using ethylcelluloses having a systematically controlled distribution of substituents and
Figure 33 Change in the degree of substitution (DS) pattern at the individual C-2, C-3, and C-6 positions for series A samples prepared from synthesized 23EC.
Kondo
Figure 34 Change in DS pattern at the individual C-2, C-3, and C-6 positions for series B samples prepared from a commercially available EC.
DS, the influence of intramolecular hydrogen bonds, within the same chiral backbone, in determining the handedness of these lyotropic mesophases was investigated [27]. Two series (A and B) of ethylcellulose samples were used in this experiment to cover the entire range of hydroxyl substitutions possible in EC. For this set A of samples (Fig. 33), all hydroxyl groups at the C-2 and C-3 positions were almost completely ethylated and only the ethyl DS at the C-6 position hydroxyl was systematically increased with increasing sample code number. The hydroxyls at the C-6 position in cellulosics easily form intermolecular hydrogen bonds, resulting in poor sample solubility in many solvents. In this series as seen in Fig. 33, samples 1 to 4, which had a DS at the C-6 position of less than 0.78, did not give clear CH2Cl2 solutions even at concentrations of 1 wt.%. A high degree of substitution at the C-6 position was required for the polymer to dissolve in CH2Cl2. For series B (Fig. 34), the DS at the C-3 position was somewhat lower than that for the other positions. The C-2 and C-6 hydroxyl groups were easily and completely ethylated to give a saturated point with a DS of 1.0. Thus only the ethyl DS for the C-3 hydroxyls was individually increased up to a limit of 1.0. In contrast to series A, the C-6 position hydroxyl groups in series B were almost completely ethylated and all samples dissolved in CH2Cl2 at 1 wt.% to yield clear solutions. Circular dichroism (CD) was used to determine the handedness of the cholesteric structure by the sign of the induced CD band that results from the selective reflection of circularly polarized light. A positive CD band corresponds to a left-handed cholesteric twist, whereas a negative CD band corresponds to a right-handed twist. Samples from series A, as shown in Fig. 33, showed a totally different behavior in cholesteric handedness from
Hydrogen Bonds in Cellulose and Cellulose Derivatives
that of series B samples. Series A samples that were prepared from 23EC have free hydroxyls only at the C-6 position. As the sample code number increases, the free hydroxyl groups at the C-6 position are gradually replaced by ethyl groups. As already noted, hydroxyl groups at the C-6 position in cellulosics contribute favorably to the formation of intermolecular hydrogen bonds and this results in poor solubility of the polymer. This can be seen for samples 1 to 4 in Fig. 33, which do not dissolve completely even in very dilute solution. Instead, they were found to swell and form gels. Samples with a DS of more than 0.8 at the C-6 position, namely, samples 5 to 9, show induced CD spectra for concentrated anisotropic solutions from 40 to 50 wt.% polymer (Fig. 33) and all are righthanded chiral nematic liquid crystals. The above results strongly suggest that the distribution of ethyl substituents among C-2, C-3, and C-6 positions of the anhydroglucose unit in EC samples can affect the cholesteric handedness of their anisotropic solutions. In particular, the substitution of hydroxyl groups at the C3 position may play an important role in determining the handedness, whereas hydroxyl groups at the C-6 position are important and contribute to the solubility of the sample in various solvents. The intramolecular hydrogen bonds formed between hydroxyls at the C-3 position and adjacent ether oxygen of the glucose ring may even be maintained in the solution state. Further, the intramolecular hydrogen bonds at the C-3 position may play a role in determining the conformation of the extended glucose chain structure, causing greater chain stiffness. Therefore once the hydroxyl groups at the C-3 position are highly substituted, then the intramolecular bonds must be cut, and the glucose unit is now freer and may rotate easily to alter the torsion angle between two consecutive units and as a result the molecular chain will be more flexible. In fact, T1 relaxation time of the C-1 carbon in a glucose unit in cellulose derivatives whose hydroxyl groups at the C-3 position remain unsubstituted is longer than that for 2,3-O-substituted cellulosics even in the solution state. 13 C NMR chemical shifts and relaxation time at the C-1 carbon also change after deuteration of the hydroxyl groups in the same system [73]. These results indicate not only the engagements of the intramolecular hydrogen bonds in the solution state, but also the positive contribution of the interaction to the molecular chain stiffness. For all samples in series A, the hydroxyl groups at the C-3 position are assumed to be almost fully substituted and thus as long as the sample is dissolved, the anisotropic solution shows right-handedness. As shown in Fig. 34 (series B), the samples with an ethyl DS of more than 0.9 at the C-3 position, EC 5 to 9, form a lyotropic righthanded chiral nematic mesophase. In relating the intramolecular hydrogen bonds at the C-3 position with chain stiffness, the above results indicate that the less stiff the chain is the more favorably the right-handed chiral nematic structure is formed. These results indicate that the contribution of intramolecular hydrogen bonds should be considered when trying to explain or account for the chiroptical properties of cellulosic mesophases.
95
II. CONCLUSION In this chapter, the author has attempted to explain the characterization of hydrogen bonds in various states from crystal to solution. It is clear that using regioselectively substituted cellulose derivatives some specific intramolecular hydrogen bonds can be characterized. However, hydrogen bonds themselves are still a very difficult subject to clarify. Further extensive study will be desired to realize the correlation between the formation of hydrogen bonds and their influence on the properties found in cellulosics. In addition, interchain hydrogen bonds in cellulosics/synthetic polymer blends [18,23,24,104] and aggregation in gels are dropped in this chapter. Of course, these subjects are of importance in terms of polymer–polymer interactions. The author could not find enough space to mention about it. We will wait for another review.
REFERENCES 1. 2. 3.
4. 5. 6.
7. 8. 9. 10. 11.
12. 13.
Jeffrey, G.A.; Saenger, W. Hydrogen Bonding in Biological Structures; Springer-Verlag, 1991, Chapters 1 and 2. Cousins, S.K.; Brown, R.M., Jr. Photoisomerization of a dye-altered h-1,4 glucan sheet induces the crystallization of a cellulose-composite. Polymer 1997, 38, 903–912. Togawa, E.; Kondo, T. Change of morphological properties in drawing water-swollen cellulose films prepared from organic solutions. A view of molecular orientation in the drawing process. J. Polym. Sci. B: Polym. Phys. 1999, 37, 451. Kondo, T.; Sawatari, C. A Fourier transform infra-red spectroscopic analysis of the character of hydrogen bonds in amorphous cellulose. Polymer 1996, 37, 393. Kondo, T.; Togawa, E.; Brown, R.M., Jr. Nematic ordered cellulose: A concept of glucan chain association. Biomacromolecules 2001, 2, 1324. Horii, F.; Hirai, A.; Kitamaru, R. Solid-state 13C-NMR study of conformations of oligosaccharides and cellulose-conformation of CH2OH groups about the exocyclic C–C bond. Polym. Bull. 1983, 10, 357. Liang, C.Y.; Marchessault, R.H. Infrared spectra of crystalline polysaccharides. I. Hydrogen bonds in native celluloses. J. Polym. Sci. 1959, 37, 385. Liang, C.Y.; Marchessault, R.H. Infrared spectra of crystalline polysaccharides. II. Native celluloses in the region from 640 to 1700 cm 1. J. Polym. Sci. 1959, 39, 269. Hermans, P.H. Physics and Chemistry of Cellulose Fibres; Am. Elsevier: New York, 1949. Marchessault, R.H.; Liang, C.Y. Infrared spectra of crystalline polysaccharides. III. Mercerized cellulose. J. Polym. Sci. 1960, 43, 71. Blackwell, J.; Marchessault, R.H. In Cellulose and Cellulose Derivatives; Bikales, N., Segal, L., Eds.; Wiley Interscience: New York, 1971 Part IV, Chapter XII, 1– 37. Marchessault, R.H.; Sundararajan, P.R. In The Polysaccharide; Aspinall, G.O., Ed.; Academic Press, Inc.: New York, 1983; Vol. 2, 12–95. Heine, S.; Kratky, O.; Porod, G.; Schmit, P.J. Eine verfeinerte Theorie der Ro¨ntgenkleinwinkelstreuung des verkna¨uelten Fadenmoleku¨ls und uhre Anwendung auf Cellulosenitrat in Lo¨sung. Makromol. Chem. 1961, 44, 682.
96 Gray, D.G. Liquid crystalline cellulose derivatives. J. Appl. Polym. Symp. 1983, 37, 179. 15. Flory, P.J. Liquid crystal polymers. Adv. Polym. Sci. 1984, 59, 1. 16. Fukuda, T. Liquid crystals of cellulosics (Japanese). Sen-i Gakkaishi 1990, 46, P-504. 17. Kondo, T. Hydrogen bonds in regioselectively substituted cellulose derivatives. J. Polym. Sci.: B, Polym. Phys. 1994, 32, 1229. 18. Kondo, T.; Sawatari, C.; St-J. Manley, R.; Gray, D.G. Characterization of hydrogen bonding in cellulosesynthetic polymer blend systems with regioselectively substituted methylcellulose. Macromolecules 1994, 27, 210. 19. Kondo, T. The relationship between intramolecular hydrogen bonds and certain physical properties of regioselectively substituted cellulose derivatives. J. Polym. Sci.: B, Polym. Phys. 1997, 35, 717. 20. Itagaki, H.; Takahashi, I.; Natsume, M.; Kondo, T. Gelation of cellulose whose hydroxyl groups are specifically substituted by the fluorescent groups. Polym. Bull. 1994, 32, 77–81. 21. Kondo, T.; Nojiri, M. Characterization of the cleavage of h-glucosidic linkage by Trichoderma viride cellulase using regioselectively substituted methylcelluloses. Chem. Lett. 1994; 1003–1006. 22. Nojiri, M.; Kondo, T. Application of regioselectively substituted methylcelluloses to characterize the reaction mechanism of cellulase. Macromolecules 1996, 29, 2392– 2395. 23. Kondo, T.; Sawatari, C. Intermolecular hydrogen bonding in cellulose/poly(ethylene oxide) blends: Thermodynamic examination using 2,3-di-O- and 6-O-methylcelluloses as cellulose model compounds. Polymer. 1994, 35, 4423. 24. Kondo, T.; Sawatari, C. Interchain hydrogen bonds in cellulose/poly(vinyl alcohol) characterized by DSC and solid-state NMR analyses using cellulose model compounds. ACS Symp. Ser. 1998, 680. 25. Kondo, T.; Sawatari, C. A Fourier transform infra-red spectroscopic analysis of the character of hydrogen bonds in amorphous cellulose. Polymer. 1996, 37, 393. 26. Itagaki, H.; Tokai, M.; Kondo, T. Physical gelation process of cellulose whose hydroxyl groups are regioselectively substituted by the fluorescent groups. Polymer. 1997, 38, 4201–4205. 27. Kondo, T.; Miyamoto, T. The influence of intramolecular hydrogen bonds on handedness in ethylcellulose/ CH2Cl2 liquid crystalline mesophases. Polymer 1998, 39, 1123–1127. 28. Sekiguchi, Y.; Sawatari, C.; Kondo, T. A gelation mechanism depending on hydrogen bonding formation in regioselectively substituted O-methylcelluloses, Carbohydr. Polym. 2003, 53, 145–153. 29. Cellulose and Other Natural Polymer Systems; Brown, R.M. Jr., Ed.; Plenum: New York, 1982; 412 pp. 30. Atalla, R.H.; VanderHart, D.L. Native cellulose: A composite of two distinct crystalline forms. Science 1984, 223, 283. 31. Sugiyama, J.; Vuong, R.; Chanzy, H. Electron diffraction study on the two crystalline phases occurring in native cellulose from an algal cell wall. Macromolecules 1991, 24, 4168. 32. Gardner, K.H.; Blackwell, J. The structure of native cellulose. Biopolymers 1974, 13, 1975. 33. Sarko, A.; Muggli, R. Packing analysis of carbohydrates and polysaccharides: III. Valonia cellulose and cellulose II. Macromolecules 1974, 7, 486. 34. Nishiyama, Y.; Langan, P.; Chanzy, H. Crystal structure
Kondo
14.
35.
36. 37. 38. 39. 40. 41. 42. 43. 44. 45. 46. 47. 48.
49. 50. 51. 52. 53. 54. 55. 56. 57.
58.
and hydrogen-bonding system in cellulose Ih from synchrotron X-ray and neutron fiber diffraction. J. Am. Chem. Soc. 2002, 124, 9074–9082. Langan, P.; Nishiyama, Y.; Chanzy, H. A revised structure and hydrogen-bonding system in cellulose II from a neutron fiber diffraction analysis. J. Am. Chem. Soc. 1999, 121, 9940–9946. Nishikawa, S.; Ono, S. X-ray diffraction of cotton cellulose fibers. Proc. Tokyo Math, Phys. Soc. 1913, 7, 131. Meyer, K.H.; Misch, L. U¨ber den Bau des krystallisierten Anteils der cellulose, V. Mitteil. Ber. 1937, 70B, 266. Fengel, D. Characterization of cellulose by deconvolution the OH valency range in FTIR spectra. Holzforschung 1992, 46, 283. Fengel, D. Influence of water on the OH valency range in deconvoluted FTIR spectra of cellulose. Holzforschung 1993, 47, 103. Fengel, D. Influence of the alkali concentration on the formation of cellulose II. Holzforschung 1995, 49, 505. Michell, A.J. Second-derivative F.T.-I.R. spectra of celluloses I and II and related mono- and oligosaccharides. Carbohydr. Res. 1988, 173, 185. Michell, A.J. Second-derivative F.T.-I.R. spectra of native celluloses. Carbohydr. Res. 1990, 197, 53. Michell, A.J. Second-derivative FTIR spectra of native celluloses from Valonia and tunicin. Carbohydr. Res. 1993, 241, 47. Marrinan, H.J.; Mann, J. Infrared spectra of the crystalline modification of cellulose. J. Polym. Sci. 1956, 21, 301. Tsuboi, M. Infrared spectrum and crystal structure of cellulose. J. Polym. Sci. 1957, 25, 159. Liang, C.Y.; Marchessault, R.H. Infrared spectra of crystalline polysaccharides: I. Hydrogen bonds in native cellulose. J. Polym. Sci. 1959, 37, 385. Marchessault, R.H.; Liang, C.Y. Infrared spectra of crystalline polysaccharides: III. Mercerized cellulose. J. Polym. Sci. 1960, 43, 71. Tashiro, K.; Kobayashi, M. Theoretical evaluation of three-dimensional elastic constants of native and regenerated celluloses: Role of hydrogen bonds. Polymer. 1991, 32, 1516. Mann, J.; Marrinan, H.J. Crystalline modification of cellulose: Part II. A study with plane-polarized infrared radiation. J. Polym. Sci. 1958, 32, 357. Ivanova, N.V.; Korolenko, E.A.; Korolik, E.V.; Zbankov, R.G. Mathematical processing of the IR spectrum of cellulose. Zh. Prikl. Spektrosk. 1989, 51, 301. Russian. Wiley, J.M.; Atalla, R.H. Band assignments in the Raman spectra of cellulose. Carbohydr. Res. 1987, 160, 113. Sugiyama, J.; Persson, J.; Chanzy, H. Combined infrared and electron diffraction study of the polymorphism of native cellulose. Macromolecules 1991, 24, 2461. VanderHart, D.L.; Atalla, R.H. Studies of microstructure in native celluloses using solid-state 13C NMR. Macromolecules 1984, 17, 1465. Kondo, T. The assignment of IR absorption bands due to free hydroxyl groups in cellulose. Cellulose 1997, 4, 281. Mare´chal, Y.; Chanzy, H. The hydrogen bond network in Ih cellulose as observed by infrared spectrometry. J. Mol. Struct. 2000, 523, 183–196. Kolpak, K.; Blackwell, J. Determination of the structure of cellulose II. Macromolecules 1976, 9, 273. Stipanovic, A.; Sarko, A. Packing analysis of carbohydrates and polysaccharides 6. Molecular and crystal structure of regenerated cellulose II. Macromolecules 1976, 9, 851. Blackwell, J. In Cellulose and Other Natural Polymer
Hydrogen Bonds in Cellulose and Cellulose Derivatives
59.
60.
61.
62.
63. 64. 65. 66. 67. 68. 69. 70.
71. 72.
73. 74.
75.
76. 77.
78.
Systems; Brown, R.M., Jr., Ed.; Plenum: New York, 1982; 412 pp. Gessler, K.; Krauss, N.; Steiner, T.; Betzel, C.; Sandmann, C.; Saenger, W. Crystal structure of h-Dcellotetraose hemihydrate with implications for the structure of cellulose II. Science 1994, 266, 1027. Gessler, K.; Krauss, N.; Steiner, T.; Betzel, C.; Sandmann, C.; Saenger, W. h-D-cellotetraose hemihydrate as a structural model for cellulose II. An X-ray diffraction study. J. Am. Chem. Soc. 1995, 117, 11397. Raymond, S.; Heyraud, A.; Tran Qui, D.; Kvick, A˚.; Chanzy, H. Crystal and molecular structure of h-Dcellotetraose hemihydrate as a model of cellulose II. Macromolecules 1995, 28, 2096. Raymond, S.; Henrissat, B.; Tran Qui, D.; Kvick, A˚.; Chanzy, H. The crystal structure of methyl h-cellotrioside monohydrate 0.25 ethanolate and its relationship to cellulose II. Carbohydr. Res. 1995, 277, 209. Gagnaire, D.; St-Germain, J.; Vincendon, M. NMR evidence of hydrogen bonds in cellulose solutions. J. Appl. Polym. Sci. Appl. Polym. Symp. 1983, 37, 261. Kondo, T.; Gray, D.G. The preparation of O-methyland O-ethyl- celluloses having controlled distribution of substituents. Carbohydr. Res. 1991, 220, 173. Kondo, T.; Gray, D.G. Facile method for the preparation of tri-O-(alkyl)cellulose. J. Appl. Polym. Sci. 1992, 45, 417. Kondo, T. Preparation of 6-O-alkylcellulose. Carbohydr. Res. 1993, 238, 231. Kondo, T. Hydrogen bonds in regioselectively substituted cellulose derivatives. J. Polym. Sci.: B, Polym. Phys. 1994, 32, 1229. Kondo, T. The assignment of IR absorption bands due to free hydroxyl groups in cellulose. Cellulose 1997, 4, 281. Blackwell, J.; Marchessault, R.H. Cellulose and Cellulose Derivatives; John Wiley and Sons: New York, 1971. Part IV. Kamide, K.; Okajima, K.; Kowsaka, K.; Matsui, T. CP/ MASS 13C NMR spectra of cellulose solids: An explanation by the intra-molecular hydrogen bond concept. Polym. J. 1985, 17, 701. Silverstein, R.M.; Bassler, G.C.; Morrill, T.C. Spectrometric Identification of Organic Compounds, Fourth Edition; John Wiley & Sons: New York, 1981; 112 pp. Dudley, R.L.; Fyfe, C.A.; Stephenson, P.J.; Deslandes, Y.; Hamer, G.K.; Marchessault, R.H. High-resolution 13 C CP/MAS NMR spectra of solid cellulose oligomers and the structure of cellulose II. J. Am. Chem. Soc. 1983, 105, 2469. Nojiri, M.; Kondo T. unpublished work. Dorman, D.E.; Roberts, J.D. Nuclear magnetic resonance spectroscopy. Carbon-13 spectra of some pentose and hexose aldopyranoses. J. Am. Chem. Soc. 1970, 92, 1355. Perlin, A.S.; Casu, B.; Koch, H.J. Configurational and conformational influences on the carbon-13 chemical shifts of some carbohydrates. Can. J. Chem. 1970, 48, 2596. Parfondry, A.; Perlin, A.S. 13C-N.M.R. spectroscopy of cellulose ethers. Carbohydr. Res. 1977, 57, 39. Dudley, R.L.; Fyfe, C.A.; Stephenson, P.J.; Deslandes, Y.; Hamer, G.K.; Marchessault, R.H. High-resolution 13 C CP/MAS NMR spectra of solid cellulose oligomers and the structure of cellulose II. J. Am. Chem. Soc. 1983, 105, 2469. Fyfe, C.A.; Stephenson, P.J.; Veregin, R.P.; Hamer, G.K.; Marchessault, R.H. Carbohydr. Chem. 1984, 3, 663.
97 79. Isogai, A.; Usuda, M.; Kato, T.; Uryu, T.; Atalla, R.H. Solid-state CP/MAS 13C NMR study of cellulose polymorphs. Macromolecules 1989, 22, 3168. 80. Horii, F.; Hirai, A.; Kitamaru, R.; Sakurada, I. Cellulose Chem. Technol. 1985, 19, 513. 81. Unpublished data. 82. VanderHart, D.L. J. Magn. Reson. 1981, 44, 117. 83. Imashino, F.; Maeda, S.; Takegoshi, K.; Terao, T.; Saika, A. Intermolecular hydrogen-bonding effect on 13C NMR shielding for enol forms of diketones in the solid state. Chem. Phys. Lett. 1982, 92, 642. 84. Horii, F.; Hirai, A.; Kitamaru, R. Solid-state highresolution 13C-NMR studies of regenerated cellulose samples with different crystallinities. Polym. Bull. 1982, 8, 163. 85. Bellamy, L.J. The Infrared Spectra of Complex Molecules; Chapman and Hall: London, 1975. 86. Hishikawa, Y.; Togawa, E.; Kataoka, Y.; Kondo, T. Characterization of amorphous domains in cellulosic materials using a FTIR deuteration monitoring analysis. Polymer. 1999, 40, 7117. 87. Hess, K.; Kiessig, H.; Gundermann, J. Z. Phys. Chem. 1941, B49, 64. 88. Hermans, P.H.; Weidinger, A. On the recrystallization of amorphous cellulose. J. Am. Chem. Soc. 1946, 68, 2547. 89. Wadehra, I.L.; St. J. Manley, R. Recrystallization of amorphous cellulose. J. Polym. Sci. 1965, 9, 2627. 90. Jezirny, A.; Kepka, S. Preparation of standard amorphous specimens for X-ray analysis of fiber crystallinity. J. Polym. Sci. Polym. Lett. Ed. 1972, 10, 257. 91. Jeffries, R. Preparation and properties of films and fibers of disordered cellulose. J. Appl. Polym. Sci. 1968, 12, 425. 92. Atalla, R.H.; Ellis, J.D.; Schroeder, L.R. Some effects of elevated temperatures on the structure of cellulose and its transformation. J. Wood Chem. Technol. 1984, 4, 465. 93. Schroeder, L.R.; Gentile, V.M.; Atalla, R.H. Nondegradative preparation of amorphous cellulose. J. Wood Chem. Technol. 1986, 6, 1. 94. Isogai, A.; Atalla, R.H. Amorphous celluloses stable in aqueous media: Regeneration from SO2–amine solvent systems. J. Polym. Sci. Polym. Chem. Ed. 1991, 29, 113. 95. Nelson, M.L.; O’Connor, R.T. Relation of certain infrared bands to cellulose crystallinity and crystal lattice type: Part II. A new infrared ratio for estimation of crystallinity in celluloses I and II. J. Appl. Polym. Sci. 1964, 8, 1311. 96. Hatakeyama, H.; Hatakeyama, T. Structural change of amorphous cellulose by water- and heat-treatment. Macromol. Chem. 1981, 182, 1655. 97. Burchard, W. Lichtstreuuntersuchungen an Polysaccharidlo¨sungen. Das Papier 1994, 48, 755. 98. Burchard, W.; Schulz, L. Functionality of the h(1,4) glycosidic linkage in polysaccharides. Macromol. Symp. 1995, 99, 57. 99. Burchard, W. Polymer structure and dynamics, and polymer–polymer interactions. Adv. Coll. Int. Sci. 1996, 64, 45. 100. Seger, B. Ph.D. Thesis, University of Freiburg, 1996. 101. Rowland, S.P.; Howley, P.S. Structure in ‘‘amorphous regions,’’ accessible segments of fibrils, of the cotton fiber. Text. Res. J. 1988, 58, 96. 102. Jeffries, R. An infra-red study of the deuteration of cellulose and cellulose derivatives. Polymer 1963, 4, 375. 103. Taniguchi, T.; Harada, H.; Nakato, K. Accessibility of hydroxyl groups in wood. Mokuzai Gakkaishi 1966, 12, 215. 104. Shin, J.-H.; Kondo, T. Cellulosic blends with
98
105.
106. 107. 108. 109. 110.
Kondo poly(acrylonitrile): Characterization of hydrogen bonds using regioselectively methylated cellulose derivatives. Polymer. 1998, 29, 6899. Yano, S.; Hatakeyama, H.; Hatakeyama, T. Effect of hydrogen bond formation on dynamic mechanical properties of amorphous cellulose. J. Appl. Polym. Sci. 1976, 20, 3221. Hatakeyama, T.; Ikeda, Y.; Hatakeyama, H. Effect of bound water on structural change of regenerated cellulose. Macromol. Chem. 1987, 188, 1875. Bikales, N.M., Segal, L., Eds.; In Cellulose and Cellulose Derivatives. Part IV, Chapter XIII; New York: John Wiley & Sons, 1971. French, A.D. In Cellulose Chemistry and its Applications; Nevell, T.P., Zeronian, S.H., Eds.; Ellis Horwood: Chichester, 1985. Chapter 3. Croon, I.; Lindberg, B. The distribution of substituents in partially methylated celluloses part 1. Svensk Papperstidn. 1957, 60, 843. Croon, I.; Lindberg, B. The distribution of substituents in partially methylated celluloses part 3. Svensk Papperstidn. 1958, 61, 919.
111. 112.
113. 114.
115. 116. 117.
Haines, A.H. Relative reactivities of hydroxyl groups in carbohydrates. Adv. Carbohydr. Chem. 1976, 33, 11. Zugenmaier, P.; Haurand, P. Structural and rheological investigations on the lyotropic, liquid-crystalline system: O-ethylcellulose-acetic acid-dichloroacetic acid. Carbohydr. Res. 1987, 160, 369. Ritcey, A.M.; Holme, K.R.; Gray, D.G. Cholesteric properties of cellulose acetate and triacetate in trifluoroacetic acid. Macromolecules 1988, 21, 2914. Pawlowski, W.A.; Gilbert, R.D.; Fornes, R.E.; Purrington, S.T. The thermotropic and lyotropic liquidcrystalline properties of acetoacetoxypropyl cellulose. J. Polym. Sci.: B Polym. Phys. 1987, 25, 2293. Guo, J.-X.; Gray, D.G. Preparation and liquid crystalline properties of (acetyl)(ethyl)cellulose. Macromolecules 1989, 22, 2082. Guo, J.-X.; Gray, D.G. Chiropitical behavior of (acetyl) (ethyl)-cellulose liquid crystalline solutions in chloroform. Macromolecules 1989, 22, 2086. Budgell, D.R.; Gray, D.G. In Polymer and Fiber Science: Recent Advances; Fornes, R.E., Gilbert, R.D., Eds.; VCH: New York, 1992; 145 pp. Chapter 12.
4 X-ray Diffraction Study of Polysaccharides Toshifumi Yui Miyazaki University, Miyazaki, Japan
Kozo Ogawa Osaka Prefecture University, Sakai, Osaka, Japan
I. INTRODUCTION The requirement for information regarding the three-dimensional structure of polysaccharides at the molecular level is growing for a number of reasons: these molecules have been regarded as biodegradable polymer materials, compared to the usual synthetic polymers; polysaccharides are the most abundant organic materials in nature; and a great variety of polysaccharides composed of various monosaccharide residues and linkages have been found. Polysaccharides can be broadly classified into three groups based on their functions, which are closely related to their occurrence in nature: structural, storage, and gel forming. Structural polysaccharides, typical examples being cellulose in plant cell walls and chitin in exoskeletons of many insects, form long fibrils or sheets which play a supporting role in various organisms. Generally, their molecular chains form extended twofold helical conformations. Storage polysaccharides characterized by highly branched chains are thought to be folded back on themselves to yield compact structures. Amylose, amylopectin, and glycogen are examples of this type of polysaccharides. The gelforming, network polysaccharides, such as alginic acids and mucopolysaccharides, which are found in the cell walls and intercellular regions of certain algae and seaweeds or the amorphous matrix material of animal connective tissues, serve as water-holding substances in these organisms. In addition, some polysaccharides have recently been found useful as biomedical materials, such as chitin/chitosan showing antibacterial action and a branched (1!3)-hD-glucan having antitumor activity. These physiologically active polysaccharides are considered to enhance the immune system systematically, resulting in antitumor and antibacterial activities.
In comparison with other biopolymers, polysaccharides are characterized by their diversity, the presence of a large number of functional groups, and their conformational rigidity. Even unsubstituted pyranoglycans contain three hydroxyl groups per sugar residue. In addition, most polysaccharides can be found in the form of linear or branched homopolymers or copolymers based on two or more different sugars as constituents. Some copolymers also result from variations of the linkage structure in the sequence of the same sugars. Several extracellular polysaccharides have more complicated chemical structures composed of one to as many as seven kinds of sugars in their chemical repeating unit. The above characteristics are easily interpreted, considering the basic stereochemical features of sugars. For example, in the case of homoglucans, the hydroxyl group at C(1) of glucose can chemically bond with one of the four hydroxyls of another glucose (i.e., 1!2, 1!3, 1!4, and 1!6 linkages), and the position of the glycosidic oxygen is either axial or equatorial to the pyranose ring (a- or hanomer), leading to two stereoisomers for each bond type. Thus polymerization of D-glucose residues provides eight types of homoglucans, each with a different glycosidic linkage structure, all of them having been found in nature. Given the fact that many kinds of sugar in pentose or hexose could form six different types of homoglycans from the former or eight from the latter, various homoglycans have been found. A theoretical treatment of the homopolysaccharide conformations was carried out by Rees and Scott [1], who proposed that the typical molecular shapes of homoglucans and other homoglycans, such as galactan, mannan, xylan, and arabinan, could be characterized in terms of four conformational types: type A—extended and ribbon99
100
like; type B—flexible and helical; type C—rigid and crumpled; type D—very flexible but, on the average, rather extended. X-ray and electron diffraction studies of various homoglycans have demonstrated that the chain conformations of these polysaccharides in crystals are reasonably consistent with the predictions of Rees and Scott [1]. The conformational rigidity of polysaccharides is revealed by inspecting the conformational probability map of the polymer where a potential energy contour map is drawn as a function of the two rotational angles of the glycosidic linkage. The allowed area for a polysaccharide where no steric overlaps occur between residues is generally much smaller than that for a polypeptide. The polyfunctional nature of polysaccharides as polyalcohols explains their ability to form a multitude of intermolecular hydrogen bonds in the solid state. Coupled with the conformational rigidity of the chains, which results in a self-ordering tendency, almost all polysaccharides readily form microcrystalline phases in the solid state, where the crystal structures are marked by extensive hydrogen-bonding network. In the x-ray structure analysis of a biopolymer, it should be noted that a polysaccharide crystal is simpler but far less complete than for a globular protein. One can obtain a single crystal of a globular protein large enough, say 0.5-mm diameter, for x-ray analysis. Even smaller crystals can be analyzed using synchrotron radiation. The number of x-ray reflections observed from the single crystal may be more than a few thousands. In contrast, a polysaccharide, as well as most of other polymers, never provides a single crystal large enough for x-ray diffraction analysis. It sometimes forms a microscopic single crystal which only can serve an electron diffraction study. The xray diffraction pattern from a polysaccharide crystal is referred to as a ‘‘fiber diagram’’ since it is diffracted from a fiber sample. A fiber sample is a polycrystalline material consisting of uniaxially oriented microcrystallites along the stretched direction of it. They are randomly oriented about the lateral directions and comprise noncrystalline region to some extent. Thus a resolution of crystal structure analysis is significantly affected by quality of a fiber diagram, depending on the degrees of crystallization and of orientation of microcrystallites. The helix axis of a molecular chain coincides with the oriented direction of microcrystallites and, consequently, of a fiber sample. In addition, there is the simplifying fact that the molecular chain axis in microcrystallites is parallel to one of the three axes of the unit cell, usually assigned to the c-axis. This axis is called the ‘‘fiber axis,’’ and the unit cell length along it is called the ‘‘fiber repeat.’’ Experimentally, the fiber repeat is readily derived from the layer line spacing of the fiber diagram. The present article describes briefly the general techniques of the x-ray fiber diffraction analysis, which includes the computer-aided model building and structure refinement methodology specialized in polysaccharide crystals. The rest of the article introduces the molecular and crystal structures of several topical polysaccharides followed by the recent advances in the cellulose crystal structures.
Yui and Ogawa
II. X-RAY STRUCTURE ANALYSIS A. Sample Preparation Some fibrous materials are naturally present as a highly oriented assembly of microcrystals, such as ramie and cotton fibers and tendon chitosan. Otherwise, the diffracting specimen for a given polysaccharide must be prepared by organizing the molecular chains. Only the fiber diagram of high quality allows one the crystal structure analysis of high resolution, and therefore a well-oriented and highly crystallized fiber sample is essential. Unfortunately, no common methodology has been established to prepare such a good fiber sample valid for all polysaccharides. The following two methods have mostly been adopted to obtain a uniaxially oriented fiber sample: spinning a fiber and stretching a film. The former is obtained by extruding a concentrated polymer solution into a precipitant solvent or solution. The latter is prepared by stretching the film cast from a polymer solution. Usually, the fiber-forming polysaccharides of the former class are able to form continuous films from their solutions as well. However, the opposite is not always true. In order to facilitate a fiber or film stretching, a polysaccharide of higher molecular weight is desirable and the films must be continuous, soft, and of low crystallinity in advance of stretching. Several methods for stretching polysaccharide film have been reported. A polymer film prepared by casting is cut into strips approximately 2 mm wide, and the strip is stretched under constant load using a weight of a few grams [2]. Another common method is to use a ‘‘stretching tool’’ by which one can manually stretch the strips. The former method requires more skills but is more likely to provide a sample of high orientation. In both cases, stretching must be performed under a desirable atmosphere, such as in air, under controlled relative humidity, in various solvents (or a mixed solvent), at a certain temperature, or under the combination of some of them, which depends on polysaccharide. Water, water– alcohol (often isopropanol) mixture, or glycerin are often used as solvent for stretching, although this aspect depends on polymer properties such as solubility. Even having obtained a well-oriented film or fiber, the sample to be x-rayed must be of high crystallinity. To improve crystallinity, the uniaxially oriented sample is annealed at a high temperature or rinsed with an acid solution, such as aqueous hydrochloride. The former procedure is done in any solvent (e.g., water), a mixed solvent (e.g., water– isopropanol), or water vapor, usually not in air, except for some polysaccharide derivatives. A sealed bomb is recommended for annealing at temperatures higher than the boiling point of the solvent. At any rate, it should be noted that there is practically no recipe to achieve successful sample preparation except for trial and error. It seems that ambivalent properties are required for the polymer material to form the oriented polycrystalline phase. For example, the film of excessive crystallinity is not appropriate for succeeding stretching. The crystallinity depends on many factors. Chemical composition in terms of polysaccharide residue and linkage type is principal.
X-ray Diffraction Study of Polysaccharides
The molecular weight (Mw) of the polymer is also essential. A low Mw is favorable for crystallization but disadvantageous for orientation, whereas high Mw is just the opposite. Other factors are the solvent, temperature, and so on. A typical example of how to solve the ambivalent problem is the case of (1!3)-a-D-glucan [3]. This glucan is not soluble in water but soluble in aqueous alkali and cellulose solvents, such as hydrazine hydride and N-methylmorpholine N-oxide–dimethyl sulfoxide. Attempts to prepare a continuous film or a well-oriented fiber from such solutions were not successful. However, the glucan was acetylated, dissolved in chloroform, and cast into film, from which a well-oriented fiber sample was obtained by stretching in hot glycerin. The fiber was deacetylated in sodium methoxide–methyl alcohol, while keeping the length of the fiber constant. The crystallinity of the regenerated glucan fiber was remarkably improved by annealing in water in a sealed bomb. The resultant sample of (1!3)a-D-glucan gave a fiber diffraction pattern of high quality [3]. In conclusion, preparation of the x-ray fiber sample requires a challenging spirit. Finally, it depends on luck, the challenger sometimes encounters polysaccharides which have never been crystallized. Knowledge of the density of the polysaccharide film or fiber to be x-rayed is necessary in order to know what kind and how many molecules are packed in the crystalline unit cell. The density measurement is performed using a mixture of two solvents which do not dissolve nor swell the polysaccharide, such as xylene and carbon tetrachloride. The powder-like samples obtained by grinding the polymer film or fiber are put into a mixture of xylene and carbon tetrachloride in a stoppered measuring cylinder in a thermostat bath at, for example, 25jC. Xylene or CCl4, as necessary, is added to the suspension until the sample settles in the cylinder. Then, the solution and the sample are of the same density, and the density of the solution is measured with a picnometer. If the density of the sample is higher than that of CCl4, a mixture of CCl4 and ethylene dibromide may be employed. Some polysaccharide deriv-
101
atives, such as (1!3)-a-D-glucan tribenzoate, are swollen or dissolved by these solvents, in which case an inorganic salt solution, such as aqueous NaI solution, can be used. A graduated glass column in which the mixture ratio (concentration gradient) of the two solvents changes continuously from the top of the column to the bottom can also serve for the density measurement. The fiber sample is put into the column top and is allowed to go down until reaching the zone with the same density; at this point, the graduation is read.
B. X-ray Fiber Diffraction Measurements The fiber diffraction diagram is usually taken using a flatfilm camera with which the diffraction beams arising through the fiber sample are collected on an x-ray photo film. When the irradiation is done in the air, the x-ray beam scattered by the air causes the occurrence of a (sometimes serious) background scattering on the x-ray film. In addition, not only polysaccharides, but also other biopolymers often have water molecules in their crystals. They often change the crystalline polymorphs with relative humidity. A good example is the case of (1!3)-h-D-glucan. As described later, the glucan exhibits both the hydrated and anhydrous polymorphs and they transform readily and reversibly to each other by changing the relative humidity in the x-ray camera [4]. Not only to avoid x-ray scattering by air, but also to control relative humidity, a box camera is recommended to use for obtaining good fiber diagrams of polysaccharides and other fibrous biopolymers. By passing humidity-controlled helium gas through the camera, the fiber diagram can be obtained under any relative humidity. A helium-gas atmosphere causes practically no background scattering because the helium atom has only two electrons. Fig. 1 shows typical x-ray fiber diagrams of the oriented crystalline samples of a polysaccharide. Although a fiber diagram corresponds to the rotation diagram of single crystals where the rotation axis coincides with the
Figure 1 Fiber diagrams of three polymorphs of chitosan. Left: tendon (hydrated) polymorph; middle: annealed (anhydrous) polymorph; right: type II form which was obtained with chitosan HCl salt.
102
Yui and Ogawa
fiber axis, it has much poorer quality than a single-crystal data. Three-dimensional reflection data are reduced to a two-dimensional pattern, generally accompanied by an overlapping of reflection peaks. The diffraction spots are broad and diminish rapidly in intensity with increasing diffraction angles due to the small size of each microcrystal. Therefore most reflections may disappear into the background scattering arising from noncrystalline regions. Disorders of arrays of microcrystals along the fiber axis cause severe arcing in a profile of diffraction spots—in particular, at larger diffraction angles. The diffraction angle, 2h, of each reflection is obtained by measuring the distance from the center of the pattern to the diffraction maximum using a comparator. Crystalline powder of sodium fluoride is lightly dusted on the sample in order to provide a calibration diffraction ring (0.2319 nm) on the fiber diagram. The spacing between adjacent reflection planes, d, and h are related by the Bragg law: nk ¼ 2dsinu;
n ¼ 1; 2; 3; . . .
where k is the wavelength of the x-ray radiation. It is sometimes difficult to define the diffraction maximum of some spots—for instance, those giving the peak profiles that unsymmetrically broaden or diffuse out in the background scattering. The former case may arise from the combined spot consisting of several diffraction peaks with the 2h values being close each other. A set of d-spacing values is then used to determine unit cell parameters (lengths of a-, b-, and c-axes and angles of a, b, and c) and the space group of a given crystal by a trial and error method. The next step is measuring the relative intensity of each reflection on a fiber diagram in order to get the structure amplitude of each reflection plane, which will be described in the next section. The intensities of diffraction peaks are generally obtained by radial scans of a microdensitometer on x-ray films to trace the diffraction maximum of each spot. The combined diffraction peaks may have to be resolved into individual peaks by the least-squares curvefitting procedure. However, when dealing with such onedimensional peak profiles, one sometimes finds that a measurement for severely deformed or arced peak is likely to result in unreasonable value. The two-dimensional scans over the whole diffraction pattern should provide more appropriate profiles of diffraction peaks; this requires a computer-controlled microdensitometer to process a large amount of digitized data. Compared with one-dimensional scanning data, further sophisticated mathematical techniques are necessary for the two-dimensional data in the background removal and the peak profile resolutions. The details of the two-dimensional collection and processing of a fiber diffraction diagram were discussed by Millane and Arnott [5–7]. As shown in Fig. 1, a large variation of the intensity of reflection from strong to weak is observed, depending on the number of electrons present on the reflection plane. However, the dynamic range of the usual x-ray photo film is around 102. Consequently, a set of films where four to five films are piled up must be used for
obtaining fiber patterns by x-ray irradiation. Then, the intensities of all the reflections appearing on all the films are measured. This procedure requires tough work and is timeconsuming, and the multiple film pack technique often provides erroneous evaluation for some of the intensities. An advance in x-ray diffraction measurement is represented by development of an imaging plate (IP) to replace the x-ray photo film [8–11]. The IP has been widely used in the x-ray analysis of a globular protein single crystal and in the synchrotron x-ray diffraction studies. The plate is a plastic disk coated with photostimulable phosphor crystals and is a new type of two-dimensional detector for x-ray beams. The diffraction pattern recorded on the IP is read by measuring the fluorescence intensity stimulated by a He– Ne laser beam, and all the data can be saved in various storage media. In addition, the plate can be used repeatedly by using an erasing machine. The IP is characterized by a wide dynamic range (106) and high sensitivity, which readily accomplishes about 10 times shorter exposure time and 10–60 times higher accuracy in measuring diffraction intensity than the use of conventional x-ray films. Particularly, the wide dynamic range of the IP provides a great advantage in measuring the fiber diffraction data where a relative intensity of each spot often varies by a factor of 103 so that only a single IP can serve for measuring the intensities of all reflections occurring from a fiber crystal. Obata and Okuyama [9–11] reported the fiber diffraction data collection and processing system using IP. The relative intensities, I0, are converted to the observed structure amplitudes, jF0j, by the equation: AF0 A ¼ ½KI0 =Lp1=2 In the equation, Lp is the Lorentz polarization correction factor for the fiber diffraction data, and the scale factor K incorporates the geometric corrections.
C. Refinement of Molecular and Crystal Structure Unlike an ordinary single-crystal structure analysis in which a large amount of reflection intensity data on order of 103–104 is available, the exact positions of individual atomic coordinates in the unit cell cannot be determined solely from the fiber diffraction data. Usually, in the case of polysaccharide crystal structures, the geometry of the sugar residue is first defined based on the structural data of relevant small molecules that have been determined by the single-crystal data. As shown in Fig. 2, with the fixed residue geometry, the helical conformation of a polysaccharide is described by either a pair of glycosidic torsional angles (U, W) and glycosidic bridge angle, s, or the rotation of an entire residue, h, around a ‘‘virtual bond’’ (an imaginary bond connecting the glycosidic oxygens). In the case of a regular helical chain model, the former parameters must be adjusted under the constraints of a set of the helix parameters: h, an axial rise per residue, and n, a number of residues per helix repeat. These values, related to the fiber repeat distance, c, such that c=hn, can be obtained directly from a measurement of meridional
X-ray Diffraction Study of Polysaccharides
103
In this equation, the first term describes the differences between observed, Fom, and calculated, Fcm, structure amplitudes, each being given the weight, Wm. The second term represents the sum of the nonbonded interaction energies, eij, that estimate stereochemical acceptability of the crystal model. The third term, Gq, is a set of constraint relationships among the parameters that are to be zero, and kq is initially undetermined Lagrange multipliers. The minimizing function installed in PS79 is ( ) X X 2 P ¼ fR þ ð1 f Þ Dk þ w eij ij
k
Figure 2 Chain conformational and helix parameters for the twofold helical chain (n=2) represented by the regular helical structure of chitin. All hydrogen atoms are omitted.
where the fractional weight, f, balances the x-ray crystallographic and stereochemical terms. In addition to the nonbonded interactions (third term), the second term also involves the bonded interactions, Dk, to evaluate the amount of deviations of any bond length, bond angle, or conformation angle from their standard values. The first term can be either the x-ray crystallographic residuals X X AAFom A AFcm AA= AFom A R¼ m
reflections of a fiber diagram. Exocyclic rotational groups, v, such as a hydroxyl methyl group on C(5) and N-acetyl and O-acetyl groups for sugar derivatives, can be rotated when necessary. Although these parameters are called chain conformational parameters, those that define the positions of an entire molecular chain in a unit cell are the chain-packing parameters. They are chain rotation about the helix axis, the z-translation of the chain along the fiber axis, and the x–y positions of the helix axis on an ab plane of a unit cell. The two representative programs that are principally aimed at studying the molecular and crystal structures of biopolymers have been developed: LALS [12] and PS79 [13]. Both programs, in addition to the ordinary procedure for x-ray diffraction analysis, are equipped with the stereochemical refinement approach to complement the fiber diffraction data of poor quality. The algorithms and background theories adopted by the programs have been described in detail by their respective authors, along with the strategies in solving polymer crystal structures [12,13]. The discussion herein will focus on the comparisons between the two methods. With regard to helix model building and its refinement, LALS uses the glycosidic linkage parameters U, W, and s to describe chain conformation, whereas PS79 adopts the virtual bond method. Either method allows a monomer geometry to vary in the course of structure analysis. The virtual bond approach of PS79 has been originally developed for solving a polysaccharide conformation. LALS is designed to be more flexible and readily applicable to the other biopolymer systems such as polypeptides and polynucleotides. The quantity of the following function is minimized in LALS: X X X Wm jFom Fcm j2 þS eij þ kq Gq V¼ m
ij
q
m
or the weighted one " #1=2 X X 2 2 RW ¼ Wm AAFom A AFcm AA = Wm AFom A m
m
These residuals are also calculated for crystal models in LALS. Minimizing these functions are carried out by the constrained least-squares process in LALS and by Complex method in PS79. The latter method performs a direct search for the minimum of a multidimensional function by evaluating the function at several trial points, while variables as well as the functions are confined within given constraints or limits. Advantages to this method, therefore, over those of PS79 in structure determination, are that the number and type of variable and their limits and constraints are readily introduced and changed in the course of the minimization. A disadvantage is that the optimization proceeds very slowly as it approaches the minima, in particular, in the final stage of the structure refinement where more variables should be involved. In spite of above differences in the model building and minimizing procedures, it was suggested that the two methods were able to produce essentially similar structures when the refinement was carried appropriately [14]. The general strategy of crystal structure analysis using the above programs is that it proceeds on a ‘‘trialand-error’’ basis. Possible crystal models are established and each is evaluated against the stereochemical restraints and the x-ray diffraction data at individual steps of the structure analysis. As the structure determination proceeds, inferior models are eliminated, and the most probable one is finally selected. The first stage of structure determination is to construct the helical model of a polysaccharide chain. As mentioned earlier, the starting geometry of a monomer residue can be taken from the
104
atomic coordinates obtained by the x-ray single-crystal studies. When appropriate experimental data are not available, the optimized structure by molecular mechanics (MM) calculations may be an alternative source of monomer geometry. As for a- and h-D-glucoses, their standard residues whose atomic coordinates were averaged from the crystal structures of several relevant sugars were proposed [15]. The chain conformation is refined by minimizing the stereochemical interactions with respect to the chain conformational parameters mentioned above, by imposing the helical symmetry defined by n and h. In the second stage, molecular chains are placed based on the information on the density of crystals and the space group suggested forms the diffraction pattern. The poor quality of diffraction pattern often prevents one from discriminating a unique space group among the possible ones. In such a case, all packing models having possible symmetries are constructed and tested. The authors of both PS79 and LALS suggested that an initial search for chainpacking parameters should proceed solely with the stereochemical constraints, not based on the x-ray diffraction data [13,16]. The primarily reason for this was that the calculations of structure amplitudes were considered to be more time-consuming than those of stereochemical functions. At present, however, such a problem becomes virtually negligible owing to the drastic development of computer hardware in the last decades. In fact, LALS, which was originally designed for a main-flame computer, can be implemented by a commonly used PC! Furthermore, because the potential surface of the steric energy is generally more complicated and consists of more local minima than that of the x-ray crystallographic residuals, R and RW, the minimum position may be more easily as well as quickly identified on the latter surface. The stereochemical search is virtually useless in determining hydrated crystal structures where the nonbonding, interchain interactions are mostly negligible due to the involvement of water molecules. It therefore seems to be more appropriate that crude structure with regard to chain-packing positions is determined by using the x-ray diffraction data. Chain rotational positions are first investigated against the hk0 diffraction data, which is followed immediately by a search of the z-translational position using the hk1 data. The stereochemical constraints should be introduced, by minimizing the total values of the above minimizing functions, in the final stage of structure refinement where the packing and conformational parameters are simultaneously refined. Care must be taken in introducing attractive interaction, such as the hydrogen-bonding interaction, into the crystal structure model. Introducing it on an improper refinement step may lead to prejudiced models. The crystal structure analysis of hydrated polysaccharides requires extra parameters for the locations of water molecules. After placement of molecular chains in the unit cell, initial x–y locations of waters are generally obtained by calculating either a difference Fourier or R factor map of the ab projection plane with the hk0 diffraction data. The latter map represents variations in R (or RW)
Yui and Ogawa
factors by placing a single water molecule on each grid point over the ab plane in turn. These x–y positions are subsequently extended to the three-dimensional case by introducing the hk1 diffraction data. Similar methodology can be applied to the case of polysaccharide salts in determining the locations of ions. An alternative method for evaluating the effect of water molecules is the use of the ‘‘water-weighted’’ atomic scattering factors [17]. This approach assumes that water molecules do not reside at defined crystallographic positions and that their electrons are smeared out throughout the unit cell. The crystal structure of curdlan hydrate introduced later was determined by combining the above methods; for 36 water molecules present in the unit cell, one-half was found at the defined positions near monomer residues, and the other half was distributed in a statistical manner [18].
III. MOLECULAR CONFORMATIONS OF TOPICAL POLYSACCHARIDES A. Polyaminosugars 1. Chitosan So far, one of the most promising polysaccharides is chitosan, a linear polymer of h-(1!4)-linked 2-amino-2deoxy-D-glucose residues, which is readily prepared from chitin by chemical N-deacetylation. Chitin, chitosan, and a partially N-acetylated chitosan have been widely developed to be used as antimicrobials, biomedical materials, cosmetics, food additives, separators, sewage disposal, agricultural materials, and so on. The chemical and biochemical reactivity of chitosan and the partially acetylated chitosan are higher than those of chitin because chitosan has free primary amino groups distributed regularly in its chain. Crystal structures of chitin had been analyzed by Gardner and Blackwell [19] for the h-chitin polymorph and by Minke and Blackwell [20] for a-chitin and have been presented in many books (e.g., Ref. [21]). The first fiber diagrams of chitin and chitosan were reported by Clark and Smith [22] in 1937. However, the first complete crystal structure of a chitosan polymorph was published in 1994 [23], although the base (ab) plane structure of chitosan crystal had been reported in 1985 [24]. So far, three crystalline polymorphs (x-ray fiber diagrams) of chitosan have been found. One, the most abundant, is called the ‘‘tendon chitosan’’ polymorph (Fig. 1 left) [25], which is prepared from chitin of a crab tendon by Ndeacetylation. It is a hydrated form found by Clark and Smith, where the chitosan molecule forms an extended twofold helix (Fig. 3a) in the crystal [26]. The second is the ‘‘annealed polymorph’’ (Fig. 1 middle) which is anhydrous [27]. Cairns et al. [28] found a different fiber pattern of chitosan but similar to that for a hydrochloride salt of chitosan [29] (Fig. 1 right), and they proposed an extended 8/5 (a left-handed eightfold) helix for the chitosan conformation. When the chitosan sample was stored at 98% relative humidity, it exhibited another pattern of the more conventional twofold helix [28].
X-ray Diffraction Study of Polysaccharides
105
hydrogen bonds contribute to stabilizing the three-dimensional structure in the crystal. The anhydrous crystal of chitosan neither dissolves in any aqueous acid solution nor forms a complex with any transition metal ion [23]. Therefore the anhydrous chitosan may be considered an inert material. The reason this polymorph is called ‘‘annealed’’ is that it has been obtained by heating a stretched chitosan film in the presence of water [27]. Later, no annealing was found to be necessary to obtain the anhydrous crystal for a chitosan sample having lower molecular weight [25]. Having a regular distribution of the aliphatic primary amino groups, chitosan exhibits a remarkable ability to form salts with acids and to form complexes with transition metal ions [28]. As shown in Table 1 [31], the crystalline polymorphs of chitosan salts with both inorganic [32] and organic [33–36] acids are divided into two types, depending on the acid used. In the case of some salts, they depend on
Figure 3 Packing structure of hydrated chitosan projected along the a-axis (a) and along the c-axis (b). Filled circles denote nitrogen atoms. For the sake of clarity, only three polymer chains of the lower layer in (b) are shown in (a). (From Ref. 26.)
As shown in Fig. 3, the chitosan molecules in the hydrated form have the twofold helical symmetry reinforced by an O(3)UO(5) hydrogen bond with the repeating period of 1.034 nm [26]. This is a typical structure for the h-(1!4)-linked polysaccharides such as cellulose, mannan, and chitin. The orientation of O(6) has a gt conformation [30]. Adjacent chitosan chains along the b-axis are arranged in an antiparallel fashion and are linked to each other by two N(2)UO(6) hydrogen bonds along the b-axis (Fig. 3a). These sheets are piled up along the a-direction (Fig. 3b). No direct hydrogen bond is present between the sheets, but the hydrogen bonds via water molecules hold the chain sheet to stabilize the whole packing structure. In the ‘‘annealed’’ polymorph, the extended twofold helical conformation of chitosan is also stabilized by intramolecular O(3)UO(5) hydrogen bonds, and an O(6) atom is rotated at near gt position as shown in Fig. 4 [23], which are the same features to those observed in the hydrated polymorph. Two chains pass through the unit cell in an antiparallel fashion. Intermolecular N(2)UO(6)
Figure 4 Projections of the crystal structure of chitosan in the anhydrous polymorph on the ab (top) and bc (bottom) base planes. All hydrogen atoms are omitted, and hydrogen bonds are shown as dashed lines. (From Ref. 23.)
106
Yui and Ogawa
Table 1 Classification of the Inorganic and Organic Acid Salts of Chitosan Type
Characteristics
Acid
Type I
Extended twofold helix (anhydrous)
Type II
Less extended twofold helix (hydrated)
HNO3 (high concentrationa), HBr, HI L-ascorbic acid L- or D-lactic acid (high temperatureb) Maleic acid HNO3 (low concentrationc), HF, HCl, H2SO4 Succinic acid Fumaric acid L-tartaric acid L- or D-lactic acid (low temperatured) Monocarboxylic (formic, acetic, or propionic) acids
a The acid concentration was 7 M at the salt preparation (Chanzy, private communication). b The salt was prepared at 50jC. c The acid concentration was 2.8 M at the salt preparation (Chanzy, private communication). d The salt was prepared at 15jC.
the preparation temperature or on the acid concentration. The type I salts provide different fiber patterns to one another, but all of them correspond to an anhydrous form and involve the unreacted chitosan chains of the extended twofold helical conformation [29]. All the type II salts indicate similar fiber patterns to that of chitosan HCl salt (Fig. 1 right). This indicates that these acid ions are not located in a regular position in each crystal [29]. Accordingly, it is not likely that the acid ions contribute to the fiber diffraction pattern. The molecular and crystal structure of chitosan–formic acid salt (a type II salt) is shown in Fig. 5 [37]. The less-extended twofold helix conformation with the tetrasaccharide repeat (fiber axis length=4.08 nm) as a helical asymmetric unit was proposed for the chitosan chain in the type II salt. There are two antiparallel chitosan chains, one at the corner and the other at the center of the unit cell (Fig. 5b). Neither acid nor water molecule has been defined because they are not arranged in a regular position in the crystal structure. This ‘‘shrinking’’ of the molecular conformation observed in the type II salts seems to be unique behavior of a chitosan chain, which has not been detected for any other h-(1!4)-linked polysaccharide, such as cellulose or chitin. The latter two exhibit the fully extended twofold helical conformation in all of their crystal forms. The regular distribution of cation, –NH+ 3 , along the chitosan chain would be a primary cause for the chain shrinking with the presence of particular anion species.
A Spontaneous Water-Removing Action of the Type II Salts An interesting phenomenon has been observed in the type II salts, in particular, with the monocarboxylic acid salts [31,34,36], which was first found for a chitosan–acetic acid salt [34]. The chitosan salt samples freshly prepared show the x-ray diagram similar to the typical type II salt (Fig. 1 right) where the chitosan chain forms the lessextended twofold helix. A completely different fiber pattern is then observed when the salt specimen is stored at room temperature of around 80% RH for 3 months. The diagram appears very similar to that of the ‘‘annealed’’ polymorph of chitosan (Fig. 1 middle). This indicates that acetic acid is spontaneously removed from the chitosan salt accompanied by water molecules present in the salt crystal, resulting in the transformation to the anhydrous crystal of chitosan. Measurements of the density and the FT-IR spectrum of the specimen also supported the crystalline transformation [34]. This change is accelerated when the salt was stored at higher humidity, e.g., at near 100% RH for approximately 1 month. When a formic acid salt of chitosan is kept at 100% RH, the crystalline transformation requires approximately 3 months. In contrast, the crystalline transformation for a chitosan propionic acid
Figure 5 Projections of the crystal structure of chitosan in the type II on the ac (a) and ab (b) base planes. All hydrogen atoms are omitted. Chitosan chains located at the corner and center of the unit cell are of opposite polarity. (From Ref. 37.)
X-ray Diffraction Study of Polysaccharides
salt proceeds faster, requiring 3 weeks. In the case of butyric acid, only the ‘‘annealed’’ pattern is observed because, probably, the transformation is too fast to detect. These results indicate that the behavior of the waterremoving action by acid depends on the hydrophobicity of it [36]. Recently, the action was found to occur in all the type II salts when they are immersed in an isopropanol– water mixture, and, in the case of the monocarboxylic acid salts, the procedure considerably accelerates the transformation compared with simply storing them in air [31]. The Crystalline Transformation of Chitosan As described earlier, the neighboring chitosan chains are arranged with antiparallel polarity along the chain sheet in the hydrated (Tendon) crystal (Fig. 6a), while the chain sheet in the anhydrous (Annealed) polymorph consists of parallel chains (Fig. 6b). The sheet–water–sheet hydrogen-bonding scheme stabilizes the three-dimensional structure of the hydrated crystal. Comparison of the chainpacking feature between the two polymorphs indicates that drastic rearrangement of chains appears to be necessary on transformation from the hydrated to the anhydrous crystal, obviously involving breaking and subsequent formation of intermolecular hydrogen bonds. This may be a possible reason for the very high annealing temperature of 240jC that is required for preparing the anhydrous polymorph of chitosan having a high molecular weight (e.g., viscosity average degree of polymerization: 10,800) [25]. Such an excessive heating causes unfavorable thermal decomposition of the chitosan sample, in particular, on the surface, and consequently provides a less inert sample of anhydrous chitosan. Therefore as an alternative approach to prepare the anhydrous or annealed chitosan
Figure 6 Crystalline transformations of chitosan. The ab planes of (a) hydrated (Tendon) and (b) anhydrous (Annealed) chitosans, and that of (c) the type II salt. Molecules with gray color are up-chain, while the others are down-chain.
107
sample, more moderate method based on ‘‘spontaneous water-removing action’’ to obtain an inert chitosan sample has been proposed [31]. Instead of adopting a direct transformation from the hydrated to anhydrous polymorphs, the procedure detours via the type II salt formation, which proceeds under room temperature throughout the process. Whereas the transformations to the anhydrous polymorph are irreversible from both the hydrated polymorph and the type II salts, the type II salt is readily converted to the original hydrated tendon chitosan by neutralization with an aqueous alkali such as sodium hydroxide solution. In the case of the type I salts, no such transformation occurs although they are stored for a prolonged period. On the contrary, all the type I salts change to the original hydrated (tendon) chitosan when they are immersed in an isopropanol–water mixture. The behavior of the type I salts is rather predictable because this is nothing more than dissociation of salt molecules in aqueous environment. Although any reasonable mechanism for the ‘‘water-removing action’’ has not currently been proposed, the phenomena may intimately be related to the stereochemical strain inherent in the chitosan chain and the crystal lattice force. The strict twofold helical conformation observed among most of h-(1!4)-linked chains is resulted from the crystal lattice force to achieve a reasonable chain packing. Such chains, partly stabilized by O(3)UO(5) intramolecular hydrogen bond, are slightly strained as an expense for the crystal packing. As obvious from Fig. 6c, the chitosan chains are loosely packed in the type II salt crystals, where the chains are relaxed into the less-extended helix. In addition, there seems to be no direct hydrogen bonding between the chains in the type II crystal. This facilitates reformation of the intermolecular hydrogen-bonding scheme for the anhydrous crystal as a result of releasing anions as well as waters. In the crystals of chitosan–transition metal complexes where the free amino groups of chitosan molecule coordinate metal ions, such as cadmium, zinc, cupric, nickel, cobalt, and mercury ions, the backbone chitosan molecule always retains the most abundant twofold helical conformation [38]. Improvements [39] of crystallinity of nine chitosan–metal salts complexes revealed that all the crystals were orthorhombic, and that the unit cell parameters (a- and b-axis lengths) depended on the counterions of the metal salt (such as SO42, Cl, AcO, and NO3) and not the metal ions. In each chitosan–metal complex, a metal ion is coordinated with an amino group of D-gluosamine dimer residues. Based on these findings a ‘‘pendant model’’ was proposed for the coordination mode of the chitosan– transition metal complexes [39] which is conflict with the ‘‘bridge model’’ proposed earlier, where four amino groups of chitosan chains coordinate one metal ion [40]. 2. Polygalactosamine Another polysaccharide consisting of amino sugar extracted from the culture fluid of Paecilomyces sp. I-1 is poly[(1!4)-a-D-galactosamine], which is a linear polymer
108
Yui and Ogawa
of a-(1!4)-linked 2-amino-2-deoxy-D-galactose [41]. This polysaccharide was found to have a flocculating action similar to that of chitosan on suspended soil in aqueous solution [42]. The configurational difference between Dglucosamine (glucose) and D-galactosamine (galactose) lies only in the geometrical position of the hydroxyl group with respect to the pyranose ring at C(4)-equatorial for the former and axial for the latter, while those of C(1) hydroxyl groups are of the opposite configurations to the respective C(4) hydroxyl configurations when these sugars are polymerized with (1!4)-linkage. Despite the significant difference in the linkage structure between the two (1!4)-linked glycans, x-ray analysis indicated that the poly[(1!4)-a-Dgalactosamine] forms the twofold helical (zigzag) conformation similar to its glucose counterpart, e.g., cellulose, but with a somewhat kinked structure (Fig. 7) [43].
B. (1!3)-B-D-Glucans Some polysaccharides are expected to work as medicines. The most topical polysaccharide medicine is a branched (1!3)-B-D-glucan, such as lentinan, schizophyllan, or scleroglucan, which exhibits an anticancer activity. Their chemical structures are almost the same: a main chain consisting of (1!3)-linked B-D-glucopyranosyl units along which there are side chains of single B-D-glucopyranosyl units attached by (1!6)-linkage to every three glucose residues of the backbone glucan chain [44]: h-D-Glcp 1 # 6 Poly½!3Þ-h-D-Glcp-ð1!3Þ-h-D-Glcp-ð1!3Þ-D-Glep-ð1! (1!3)-h-D-Glucan has been of interest not only for the food industries as a food additive, as it forms a strong gel [45] in the presence of water, but also for basic research because of its unique conformation, a triple helix. This glucan has been studied by Marchessault et al. [4,18,46] and Bluhm and Sarko [47]. All of their x-ray results indicated
Figure 7 Twofold poly[(1!4)-a-D-galactosamine] helix, projected perpendicular (top) and parallel (bottom) to the chain axis. The striped balls are nitrogen atoms. All the hydrogen atoms are omitted. (From Ref. 43.)
Figure 8 Projection of the triple helix of (1!3)-h-D-glucan in the anhydrous polymorph on the xz (top) and xy (bottom) planes. Dashed lines are intrahelix hydrogen bonds. Hydrogen atoms are omitted. (From Ref. 46.)
that this glucan constructs triple-helical conformations in the crystal. Two polymorphs have been found for the triplex, anhydrous and hydrated, which transform reversibly from one to the other by changing relative humidity; 20% RH is the boundary. Fig. 8 shows the molecular structure of the glucan in the crystal of the anhydrous polymorph [46]. The intramolecular hydrogen bond stabilizing the 6/1 helix of each strand was not detected; the original distance between O(5) and O(4) atoms, 0.318 nm, was possibly indicative of hydrogen-bonding formation. As shown in Fig. 8 (bottom), the three strands of the triplex are linked together through triads of strong interstrand hydrogen bonds between the O(2) hydroxyls (distance: 0.272 nm) stabilizing the triplex structure. All the O(6)
X-ray Diffraction Study of Polysaccharides
hydroxymethyl groups of the glucose residues are outside of the cylinder of the triple-helical structure. Therefore in the case of the branched (1!3)-h-D-glucan, the glucose residues of the side group attached at the O(6) position of every three glucose residues of the backbone (1!3)-h-Dglucan may be located further outside of the cylinder. This suggests that the side group of the branched (1!3)-h-Dglucan may not disturb the triple-helix formation of the
109
backbone glucan. In the case of the hydrated polymorph (Fig. 9), the crystal structure and the triplex are very similar to those of the anhydrous polymorph, and hydration simply expands the unit cell, permitting the water to enter the intertriplex spaces [18]. It has been found that (1!3)-h-D-glucan exhibits single-stranded sixfold or sevenfold helical conformations in crystals [48,49]. Okuyama et al. [50] proposed the single
Figure 9 Top: Stereo views of the triplex of (1!3)-h-D-glucan in the hydrated polymorph. Bottom: Projection of the crystal structure in the ab plane. Hydrogen atoms are not shown and water molecules are indicated by filled circles. Hydrogen bonds are drawn with dashed lines. The O(6) atoms of all 18 residues are numbered. (From Ref. 18.)
110
right-handed sixfold helical conformation of the glucan (Fig. 10) in the highly hydrated crystal, in which water content was more than 70 wt.% in the unit cell. This single helix is considered to be stabilized with a weak intramolecular hydrogen bond between O(5) and O(4) of the next glucose residue (distance: 0.314 nm) [50]. Therefore this helix may be stabilized by the water molecules present in the unit cell. After finding the triplexes of (1!3)-h-D-glucan, relatively similar x-ray fiber diagrams of the branched (1!3)h-D-glucan, scleroglucan, were obtained, suggesting that the backbone chain formed a triple helix similar to that of (1!3)-h-D-glucan [51]. In fact, an x-ray analysis of schizophyllan revealed the triple-stranded right-handed, 6/1, helical conformation as shown in Fig. 11 [52]. All the side glucose residues are located outside of the triplex of the backbone glucan chain, indicating that the side chain does not disturb the backbone triplex formation. In water solution, the polysaccharide also forms a triple-stranded helix [53]. Interestingly, the antitumor activity is considered to require the triple-helical conformation of schizophyllan [54]. Single crystal structure analysis of oligosaccharides provides the unambiguous knowledge of the conformations of glycosidic bonds (U, W) and exocyclic groups that may be applicable for further interpretation for the corresponding polysaccharide structures. As shown in Fig. 12, Okuyama and Noguchi [55] suggested, by surveying the crystal structures of the (1!3)-h-linked oligosaccharides, that the U–W conformations of the acetyl oligosaccharide (compounds A–F) were found in the same potential well as those of the polysaccharides (compounds I–III [50]). It should be noted that this group of acetyl oligomers also involves the acetyl trisaccharide with (1!6) branching acetyl glucose residue (compound F, Fig. 13)
Yui and Ogawa
Figure 11 Molecular structure of schizophyllan, projected perpendicular (top) and parallel (bottom) to the chain axis. (From Ref. 52.)
whose structure has been determined by Noguchi et al. [56]. On the other hand, the conformations of the nonsubstituted and nonacetylated disaccharides (compounds L and M, respectively) belong to a different potential well which corresponded to a considerably large, left-handed helix chain (n=14–17). Obviously, such a large helix should be unstable as a regular conformation, unless the chain includes a small molecule inside the helix. In the disaccharide crystal, the intermolecular packing force appears to be more dominant in determining the glycosidic conformations.
C. (1!3)-a-D-Glycans
Figure 10 Molecular and crystal structure of the single helix of (1!3)-h-D-glucan. (From Ref. 50.)
1. (1!3)-a-D-Glucans Streptococcus mutans, a bacteria isolated from human saliva, produces a water-insoluble a-D-glucan from sucrose. This glucan forms dental plaque and, consequently, contributes to dental caries. The chemical structure of the glucan consists of a backbone (1!3)-linked a-D-glucan chain with side chains of a-D-glucose residues attached on the O(6) position of the backbone chain. The insolubility property is attributable mainly to the linear, (1!3)-linked backbone chain, whereas the (1!6)-linked side chains are related to the adhesion of the D-glucan to the surface of teeth, hydroxyapatite [57]. Another, but noncariogenic, water-insoluble a-D-glucan is produced by Streptococcus salivarius which is also isolated from human saliva and has a similar backbone chain, (1!3)-a-D-glucan, but the side
X-ray Diffraction Study of Polysaccharides
111
chains attached on O(6) of the backbone are longer than those of the mutans glucan. They consist of D-glucose residues linked by (1!3)-, (1!4)-, and (1!6)-linkages [58]. The molecular and crystal structures of the backbone (1!3)-a-D-glucan, which was prepared from the salivarius glucan, in its dry form were determined by x-ray analysis (Fig. 14) [3,59]. The chain conformation of the glucan is nearly completely extended, and it is a twofold helix (i.e., a zigzag structure). An intramolecular O(2)UO(4) hydrogen bond stabilizes the conformation, and extensive intermolecular hydrogen bonds stabilize the sheetlike structure, with an alternating polarity of chain directions (antiparallel fashion) within the sheet. In addition to this dry form of (1!3)-a-D-glucan, two hydrated polymorphs have been reported by Jelsma and Kreger [60,61]. They obtained fiber patterns of these polymorphs using a (1!3)-a-D-glucan from a fungus, Laetiporus sulphureus (Bull ex. Fr.) Murrill. Although these fiber patterns have not been analyzed completely, it is clear that the glucan conformation in each
Figure 12 Distribution of the glycosidic conformations (A, C) of (1!3)-linked oligosaccharides and (1!3)-h-linked polysaccharides; A=O(5)UC(1)UO(1)UC(3) and C=C(1)U O(1)UC(3)UC(2). Broken and solid lines denote iso-n and iso-h contours, respectively. Iso-energy contours, shown in dotted lines, are drawn at interval of 1 kcal/mol above the absolute minimum. L: h-laminaribiose; M: methyl-h-laminaribioside; A: methyl hepta-O-acetyl-a-laminaribioside; B: octa-O-acetyl-h-laminaribiose; C: octa-O-acetyl-a-laminaribiose; D: methyl hepta-O-acetyl-a-laminaribioside; E: methyl hepta-O-acetyl-1-thio-h-laminaribioside; F: the compound given Fig. 15; I: curdlan form I; II: curdlan form II; III: curdlan form III; Ac: curdlan triacetate. (From Ref. 55.)
Figure 13 Chemical structure of (2,3,4,6-tetra-O-acetyl-h-Dglucopyranosyl)–(1!3)-[2,3,4,6-tetra-O-acetyl-h- D-glucopyranosyl)–(1!6)]-(2,4-di-O-acetyl-h- D-glucopyranosyl)– (1!3)-1,2,4,6-tetra-O-acetyl-h-D-glucopyranose.
Figure 14 Projections of the structure of (1!3)-a-D-glucan on ac plane (top) and ab plane (bottom) in the dry form. All hydrogen atoms are omitted, and hydrogen bonds are shown as dashed lines. The atoms of the asymmetric unit are numbered. (From Ref. 59.)
112
crystal is an extended twofold helix similar to that of the streptococcal (1!3)-a-D-glucan. Viscosity measurements and the polymorphic behavior of (1!3)-a-D-glucan from these three origins (i.e., two bacterial and one fungal glucans) suggested that the backbone glucan produced by S. mutans has the lowest length (molecular weight), and unlike other two glucans, the glucans are always crystallized in the dry form at any relative humidity from 0% to 100%; in other words, the zigzag sheet of the backbone (1!3)-a-D-glucan of the S. mutans glucan is the most stable. This may be one of the reasons why this a-glucan can stick to the surface of teeth [62]. 2. (1!3)-a-D-Mannan (1!3)-a-D-Mannans are found as backbone chains of branched heteropolysaccharides in the fruit bodies of some edible mushrooms, such as Auricularia auricula-judae (Kikurage) [63] and Tremella fuciformis Berk (Shirokikurage) [64]. The configurational difference between D-glucose and D-mannose is only in the disposition of the hydroxyl group at C(2)-equatorial for the former and axial for the latter. Because the position of the hydroxyl group at C(2) is not related to the glycosidic linkage structure, (1!3)-a-Dmannan is expected to have a similar conformation with (1!3)-a-D-glucan. Fig. 15 shows the molecular and crystal structure of (1!3)-a-D-mannan [65]. As expected, the chain conformation of the mannan is an extended twofold
Yui and Ogawa
helix similar to that of (1!3)-a-D-glucan: both structures are stabilized by the O(2)UO(4) intramolecular hydrogen bonds. These common features support the hypothesis that the chain conformation in polysaccharides tends to be governed more by its type of linkage rather than by the residue. In the crystalline unit cell, the mannan chains pack with antiparallel polarity and are connected by interchain hydrogen bonds that form an infinite, zigzag sheet. There are 16 water molecules in the unit cell, embedded between the sheets. It should be noted that the regenerated fiber samples of both (1!3)-linked a-D-glucan and a-D-mannan were obtained by the similar procedure: both involve annealing the stretched films in the presence of water. Only the mannan crystal comprises water molecules, as shown in the projections of Fig. 15, and exhibits the loosely packed appearance of molecular chains. No direct interaction exists between the chains.
D. Food Additives Polysaccharide gums have been used in the food industry as thickeners, stabilizers, suspending materials, gelling agents, emulsifiers, lubricants, films, and so forth. Xanthan and gellan are topical materials in both research and industrial purposes. All the polysaccharides introduced herewith have the ability to form gels. 1. Xanthan Xanthan, produced by a bacteria, Xanthomonas campestris, is an acidic polysaccharide and is a heteropolymer composed of the following large chemical repeating unit: Poly½!4Þ-h-D-Glcp-ð1!4Þ-h-D-Glcp-ð1! 3 z 1 h-D-Manp-ð1!4Þ-h-D-GlcpA-ð1!2Þ-a-D-Manp-6-OAc 6 4 H3 C-C-COOH Xanthan is commercially important because of the following reasons: it dissolves in cold water, the aqueous solution shows a thixotropy, and its viscosity is insensitive to variation of temperature. Based on a fiber pattern of high quality, Okuyama et al. [66] determined xanthan conformation in the crystal. As shown in Fig. 16, the xanthan chains are aligned with an antiparallel right-handed fivefold (5/1) double helix which is stabilized by four intramolecular bonds and one intermolecular hydrogen bond [66].
Figure 15 Projections of the structure of (1!3)-a-Dmannan on ab plane. All hydrogen atoms are omitted and hydrogen bonds are shown as dashed lines (top). Stereo views of the structure on bc plane (bottom). Open circles are water molecules. (From Ref. 59.)
2. Gellan Gellan gum is an extracellular polysaccharide derived from Pseudomonas elodea. The alkali-treated gellan has been widely utilized in food industry and biotechnology because it forms a transparent gel which is heat-resistant and its gel strength is less dependent on pH in comparison with other polysaccharide gels. It is a linear anionic heteropolysac-
X-ray Diffraction Study of Polysaccharides
113
ylate group (Fig. 17) [68]. Gellan salts with the monovalent cation, such as lithium or potassium, form stiff gels and that with divalent cation, Ca2+, make a more rigid gel. Based on their x-ray analysis of gellan potassium salt, Chandrasekaran and Thailambal [69] revealed that in the crystal of the potassium salt, double helix–potassium– water–potassium–double helix interactions promote the aggregation of molecules and subsequent gelation. Furthermore, they extrapolated these results by computer modeling to the calcium salt and revealed that Ca2+ ions intervene in direct and strong double helix–calcium–double helix interactions [69]. The native gellan has L-glycerate groups at C(2) on all the (1!3)-linked h-D-glucose residues in the backbone chain and O-acetyl groups at O(6) on half of them [70]. It forms a weak gel in water, but after treatment with alkali, the gum forms a rigid gel. Before the precise chemical
Figure 16 The 5/1 antiparallel double helix of xanthan viewed perpendicular to the helix axis. (From Ref. 66.)
charide composed of the following tetrasaccharide repeating unit containing a D-glucuronic acid: Poly½! 3Þ h D Glcp ð1 ! 4Þ h D GlcpA ð1 ! 4Þ h D Glcp ð1 ! 4Þ a L Rhamp ð1 ! Fiber diffraction analyses [67,68] revealed that the two lefthanded, threefold helical chains are organized in parallel fashion in an intertwined double helix and that the duplex is stabilized by interchain hydrogen bonds at each carbox-
Figure 17 Side view of the double helix of gellan in stereo showing the OHO hydrogen bonds within the molecule. Intrachain H-bonds are indicated by thin, dashed lines and interchain H-bonds by thick, dashed lines. (From Ref. 68.)
114
Yui and Ogawa
structure of native gellan was found, the acetic ester had been thought to disturb the stiff gel formation of native gellan. However, Kuo et al. [70] found that the glyceric ester was the major cause of the difference in gelation, rather than the acetic ester. This assertion was supported by a modeling calculation for native gellan potassium salt [69]. 3. Beijeran Recently, an acidic polysaccharide was found, showing a gelation property similar to gellan. The polysaccharide, designated beijeran, was excreted by the newly isolated bacteria Azotobacter beijerinckii YNM 1 and is expected to have potential applications in the food and cosmetic industries [71,72]. Beijeran is a linear polymer consisting of (1!3)-linked D-galacturonic acid, L-rhamnose, and Dglucose residues. Although all the glucose residues in the chain are O-acetylated at C6, the backbone chain is built up by the following trisaccharide sequence [71,72]: Poly½! 3Þ a D GalpA ð1 ! 3Þ h L Rhamp ð1 ! 3Þ a D Glcp ð1 ! The chemical structure is different and simpler, but beijeran has a similar function to gellan; that is, the alkali-treated beijeran forms a strong gel when reacted with calcium ion. However, the gelation mechanism appears to be different. The alkali treatment causes deacetylation of the O-acetyl groups, and the deacetylated beijeran forms gel in water in the presence of a divalent metal ion, such as Ca2+ and Zn2+, rather than a monovalent cation [71,72]. A welldefined x-ray fiber diffraction patterns of both calcium and sodium salts of beijeran have been obtained [73,74], and a complete analysis of the latter was done by Bian et al. [75] recently. As shown in Fig. 18, the beijeran molecule forms the extended twofold helix with the trisaccharide unit as a symmetric unit. The beijeran chain spirals around the molecular axis with a right-handed twist. Two beijeran chains are nestled tightly in the monoclinic unit cell of dimensions a=1.272, b=1.141, c (fiber axis)=2.462 nm, and c=123.7j in an antiparallel fashion. They are connected at their carboxylate groups by sodium–water– sodium bridges. As seen in Fig. 19, there is no room for any guest molecule to sit in or pass through this polymer sheet. All the sodium ions and water molecules are embedded between the sheets and none elsewhere. Altogether, they glue the sheets to form a well-knitted network. This could explain beijeran’s abilities for water holding and formation of oxygen-impervious films. 4. Konjac Glucomannan Konjac glucomannan (KGM) is a major component of konjac flour, a traditional food in Japan, produced from the tubers of Amorphophallus konjac C. Koch [76], and it also forms a stiff gel. Glucomannans, copolymers of Dmannose and D-glucose, have sequences of h-(1!4)-linked
Figure 18 Interhelical interactions of beigeran sodium salt in the unit cell. The sodium ions are shown as filled circles and water molecules are numbered. Dashed lines are hydrogen bonds. (From Ref. 75.)
mannan, and both linear and branched glucomannans are present. Among these glucomannans, KGM has the highest molecular weight (degree of polymerization: 6000) [76] and the highest glucose content (mannose/glucose ratio=1.6) [77]. It is a linear copolymer where h-(1!4)linked mannose sequences of the chain are at most pentameric in length, and these short segments are connected with only D-glucose or cellobiose units through h-(1!4) linkage. A well-defined fiber diagram of KGM was obtained by the acetylation–deacetylation procedure described in the case of (1!3)-a-D-glucan in ‘‘Sample Preparation’’ [78]. The diagram was very similar to that of the mannan II (hydrated) polymorph of (1!4)-h-D-mannan [78,79]. A similar result was obtained by an electron diffraction study on a single crystal of KGM [80]. Based on the x-ray fiber diagram, the crystal and molecular structure of KGM was proposed as shown in Fig. 20 [79]. The chain conformation of KGM is a twofold helix stabilized by intramolecular O(3)UO(5) hydrogen bonds, with the O(6) rotational position at gt [30]. The adjacent KGM chains are packed in an antiparallel fashion, and intermolecular hydrogen bonds occur exclusively between chains and water molecules, establishing the three-dimensional hydrogen-bond network in the crystal structure. The glucose residues replace mannose without changing the dimensions of the mannan-type unit cell, referred as an isomorphous replacement, although some disorder appears possible. The local formation of alternating gg–gt O(6) rotational position [30] may describe the disorder region due to the glucose-rich part of KGM chain in the crystal.
X-ray Diffraction Study of Polysaccharides
115
Figure 19 Packing arrangement of helices in the monoclinic lattice. Seven unit cells shown in the c-axis projection highlight the formation of sheets along the short diagonal. Water molecules (numbered) and sodium ions (filled circles) hold the sheets together by hydrogen bonds and ionic interactions. (From Ref. 75.)
IV. RECENT PROGRESS IN CRYSTAL STRUCTURE STUDIES ON CELLULOSE ALLOMORPHS Cellulose, a linear (1!4)-linked h-D-glucopyranose residue, is the major structural component of all plant cell walls and the largest biomass on earth; more than 104 tons of cellulose are produced in every year. It exists as a highly crystalline microfibril in all higher plants and some bacteria, fungi, and algae. The crystal structures of the cellulose microfibrils as well as those of the ‘‘manmade’’ fibers have been the subject of the intensive diffraction studies for almost a century. The native crystalline form, originally referred as cellulose I, converts to the second crystalline form or cellulose II by regeneration or mercerization of native cellulose fibers. The other crystalline forms known as cellulose III and IV are also derived from both cellulose I and II by treatment with liquid NH3 and successive heating in glycerol to 260jC. The realistic molecular packing scheme of cellulose I was first proposed more than 70 years ago [81]. The detailed crystal structures of these cellulose allomorphs with atomic resolution have been reported since the mid-1970s, which was promoted by the development of the fiber diffraction technique combined with the
computer modeling. Sarko and Muggli [82] and Gardner and Blackwell [83] independently proposed the crystal structure models of the native Valonia cellulose I, and Woodcoock and Sarko [84] reported the Ramie cellulose I structure. The same two groups, Stipanovic and Sarko [85] and Kolpak and Blackwell [86], subsequently established the crystal structures of cellulose II by analyzing the x-ray diagrams of rayon fibers. These studies reached the same conclusions with regard to chain directionality in the cellulose allomorphs. Whereas the cellulose chains are aligned in the same direction in the cellulose I structure, or ‘‘parallel chain,’’ they are arranged with alternative directions in the cellulose II structure, or ‘‘antiparallel chain.’’ Thus this readily explains the irreversible transition from cellulose I to cellulose II which accompanies the significant rearrangement of the chain polarity from the parallel chain to the antiparallel chain.
A. Cellulose I The three cellulose I models [82–84] exhibit similar structural features with regard to the molecular conformation and the chain-packing arrangement. The twofold helix conformation is stabilized by intramolecular O(3)HUO(5)
116
Figure 20 Projections of the structure of konjac glucomannan on ab plane (top) and bc plane (bottom). All hydrogen atoms are omitted and hydrogen bonds are shown as dashed lines. Dotted circles are water molecules. (From Ref. 79.)
hydrogen bond over the glycosidic linkage. All hydroxymethyl groups adopt a tg orientation [30]. The two chains of the parallel polarity pass through the monoclinic unit cell with the P21 symmetry. The intermolecular O(2)UO(6) hydrogen bonds connect adjacent chains to form the chain sheet. A major difference among the three models is the chain directionality with respect to the c-axis; while the Gardner and Blackwell model corresponds to the ‘‘parallelup’’ structure, the two others correspond to the ‘‘paralleldown’’ structure [87]. It has been well known that the native celluloses slightly differ among their origins. There are three reflections in the Valonia x-ray diffraction data that cannot be indexed with the two-chain monoclinic unit cell. A possible interpretation of this is to double the ab dimensions to the eight-chain monoclinic unit cell [88], which, however, introduces formidably complicated chain-packing schemes and variation of a chain conformation within the unit cell. In the previous studies based on the two-chain unit cell, therefore, the cellulose I structures were determined as an approximation to the Valonia crystal [81,82]. VanderHart and Atalla [89,90] proposed much clearer understanding of a crystalline system of cellulose I based on the result of high-resolution solid-state 13C NMR measurements. The multiplicities were shown in resonance for C4, C6, and C1
Yui and Ogawa
carbons, whose intensity patterns varied among the several cellulose samples. These results suggest that the native cellulose crystals consist of the two crystalline forms, designated Ia and Ih, and that their relative amounts depend on the cellulose origin; while Valonia and Acetobacter celluloses are rich in cellulose Ia, cellulose Ih may be major constituent in cotton and ramie celluloses [90,91]. This crystalline scheme of the native cellulose was further studied by electron microdiffraction analysis [91–93]. Sugiyama et al. classified the diffraction diagram of some algal celluloses into two distinct crystalline phases. The diagram of a major phase representing the Ia crystalline form is indexed with the one-chain triclinic unit cell, and the rest is interpreted as the two-chain monoclinic unit cell of the Ih phase. As obvious from the unit cell dimensions, the Ih crystalline form was once considered as the conventional cellulose I form. The Ia phase is transformed into the Ih phase by the alkaline hydrothermal treatment, suggesting that the latter has more stable form. The twophase system of the cellulose microfibrils allows a full indexation of their fiber diffraction diagrams, instead of adopting the eight-chain unit cell. This finding of the cellulose I allomorphism has promoted the further attempts to define the subclass structures. French et al. [94–96] studied possible chain-packing schemes of the cellulose allomorphs using the molecular modeling techniques on the basis of the established crystal formations such as the unit cell geometry and the space group symmetry. These studies indicated that the models having the parallel-up chains and a tg orientation of the hydroxymethyl group are most likely in both the cellulose Ia and Ih allomorphs [95,96]. The structure of the cellulose Ih model is essentially identical to that of the conventional cellulose I, and it is more stable than the Ia model by 0.4 kcal/mol of cellobiose units calculated from the potential energy calculations [96]. Heiner et al. [97] proposed more reasonable amount of 2.1 kcal/mol based on the molecular dynamics calculations. The latter value explains a complete conversion from Ia to Ih on a hydrothermal treatment. Recently, a more primary approach to predict the native cellulose structures was presented by Vie¨tor et al. [98], where the prediction was made by the chain pairing procedure without any crystal information. In the study, the two best chain-packing models were found to be the triclinic- and monoclinic-type arrangements having the unit cell dimensions and the symmetry close to those reported for either the cellulose Ia or Ih allomorphs. The molecular modeling studies also suggested that the conversion of the cellulose allomorphs could be reasonably explained by slipping of the chain sheets with respect to the neighboring chain sheet along the fiber axis [96,98]. Finkenstadt and Millane [99] reanalyzed the two sets of the x-ray diffraction data provided by Sarko and Muggli [82] and Gardner and Blackwell [83] as a representative of the cellulose Ih data. In order to obtain a definitive structure, this structure analysis was carried out more exhaustively than the preceding studies, where the geometries of the two residues in the asymmetric unit were varied independently while assuming both the parallel-up and
X-ray Diffraction Study of Polysaccharides
117
parallel-down models. These conditions had not been considered previously due to the limited computing resources available in those days [82,83]. This work showed that while some structure features such as a hydrogenbonding scheme and a chain conformation are essentially the same with those of the previous models, both the two x-ray diffraction data definitively prefer the parallel-up model. The projections of the final cellulose Ih model are depicted in Fig. 21.
Figure 22 A schematic representation of the hydrogen bonds in the origin (top) and center (bottom) sheets of cellulose Ih. Only the oxygen atoms involved in hydrogen bonding are labeled with clarity. (From Ref. 100.)
Figure 21 Views of the revised structure of cellulose Ih (a) obliquely to and (b) along the c-axis. Thin lines show hydrogen bonds. The hydrogen atoms are excluded from part (a) for clarity. (From Ref. 99.)
Recently, for the first time, Nishiyama et al. [100] reported a set of the full atomic coordinates of cellulose Ih, using the combined synchrotron x-ray and neutron diffraction analyses with a resolution of better than 1 A˚. In this study, the Finkenstadt and Millane models were subjected to the fully optimized structure refinement including restrained refinement of bond lengths and angles to determine the C and O atom positions against the x-ray diffraction data. The neutron diffraction data were obtained from the deuterated cellulose Ih sample (D-cellulose-Ih) as well as from the ordinary sample (H-cellulose-Ih). The former was prepared by intracrystalline deuteration of the cellulose Ih microcrystals for replacing the six independent hydroxyl hydrogen atoms in the asymmetric unit. The deuterium atom locations were identified examining the Fourier difference synthesis derived from the electron density maps between the D-cellulose-Ih and the H-cellulose-Ih. The difference density peaks could be definitively identified with possible D-O(3) positions, but D-O(2) and D-O(6) positions were less well defined. These results provided the two alternative patterns in deuterium positions for each of D-O(2) and D-O(6) atoms. Such ambiguities in positioning of some deuterium atoms yielded the two types of hydrogen-bonding schemes, designated A and B, as displayed in Fig. 22. In the hydrogen-bonding network A, which corresponds to the major one, both the origin and center chains involve the intramolecular O(3)UDUO(5) and O(2)UDUO(6) hydrogen bonds and the origin chain forms an additional O(2)UDUO(1) bond. The intermolecular O(6)UDUO(3) hydrogen bonds connect the same type of chains to construct the chain sheets and the center chains are further bound through the
118
O(6)UDUO(2) bond. On the other hand, the hydrogenbonding network B, consisting of the deuterium atoms with lower occupancies, indicates that both the origin and center chains involve the same intramolecular hydrogen bonds of O(3)UDUO(5), O(6)UDUO(2), and O(6)UDUO(1). A sheet formation only occurs in the center chains stabilized by the intermolecular O(2)UDUO(6) hydrogen bond, whereas no hydrogen bond is present among the origin chains. There is no intersheet OUHUO hydrogen bond in both the hydrogen-bonding networks, which is in accord with the previous structure analyses [82–84]. The chain sheets therefore are held together by hydrophobic interactions and weak CUHUO hydrogen bonds.
B. Cellulose II The two cellulose II models proposed by Stipanovic and Sarko [85] and Kolpak and Blackwell [86] are virtually identical, and an apparent difference in the chain arrangement is caused by the definition of chain positions. As is the same with the cellulose I chain, the two chains of the twofold helix conformation are packed with an antiparallel fashion in the monoclinic unit cell with the P21 symmetry. Both the ‘‘up’’ corner and ‘‘down’’ center chains form the intramolecular O(3)UO(5) hydrogen bond, and, according to the definition of Kolpak and Blackwell, the center chain only involves an extra hydrogen bond at O(6)UO(2), as a result of the hybrid orientations of the hydroxymethyl groups being gt and tg for the corner and center chains,
Yui and Ogawa
respectively. The corner chains construct the chain sheet connected by the interchain O(2)UO(6) hydrogen bond and their O(2) atoms also involve the O(2)UO(2) bond in the 110 plane with the neighboring center chain. A sheet formation also occurs in the center chains along the 020 plane, consisting of the interchain O(3)UO(6) hydrogen bond. The crystal structure model of Stipanovic and Sarko [85] exhibits an additional interchain intersheet O(6)UO(3) hydrogen bond. Thus as suggested by more intensive hydrogen-bonding scheme, the cellulose II crystal is energetically more stable allomorph than the cellulose I crystal. The next objective in exploring the cellulose II structure was to study the single crystal structure of h-Dcellotetraose hemihydrate as a model crystal for cellulose II [101–103]. There are some resemblances between the cellotetraose hemihydrate and the cellulose II crystals. The unit cell of h-D-cellotetraose hemihydrate contains two independent molecules, which are arranged with antiparallel polarity. In fact, one can draw the subcell inside the unit cell, which is nearly identical to the unit cell of cellulose II [102]. Likewise, the intermolecular hydrogen bonds are formed between the antiparallel molecules as well as between the parallel molecules, and they correspond to the intersheet and intrasheet hydrogen bonds in the cellulose II structure, respectively. Notable features in h-D-cellotetraose molecules are that the orientations of all hydroxymethyl groups are gt, and that one molecule is more sterically strained than the other as indicated by the puckering parameters of the D-glucopyranoses. The same
Figure 23 Views of the revised structure of cellulose II (bold line) superimposed over that of Kolpak and Blackwell model (thin line). The short O–O distances that correspond to hydrogen bonds are given by dashed lines. (A) Projection in ab plane. (B) Projection of the 1–3 molecules parallel to the c-axis. (C) Projection of molecules 4 and 5 parallel to the c-axis. (From Ref. 104.)
X-ray Diffraction Study of Polysaccharides
Figure 24 A schematic representation of the hydrogen bonds in cellulose II. Only the oxygen atoms involved in hydrogen bonding are labeled with clarity. (From Ref. 105.)
two groups engaged in the structure analysis of h-Dcellotetraose hemihydrate successively attempted to reanalyze the cellulose II structure [102,104] using the published x-ray diffraction data [85,86]. Both the two groups established the initial molecular chain structures based on their respective h-D-cellotetraose structures [102,104] and, as for one group, partly on the methyl h-D-cellotrioside structure [104]; each of two independent molecules in the cellodextrin crystals was applied to either origin or center chain of the cellulose II structure. Gessler et al. [102] concluded that both the gt/tg hybrid model as observed in the original cellulose II structures and the all-gt model based on the single crystal structure are equally likely. On the other
119
hand, according to the results of Raymond et al. [104], preference was given to the all-gt model, which accompanies significant strain on the D-glucopyranoses of the center chain. Fig. 23 compares the crystal structure proposed by Raymond et al. with that of the original Kolpak and Blackwell model. A complete scheme of the cellulose II structure was defined by the neutron diffraction analysis [105] and later complemented by the synchrotron x-ray diffraction analysis [106]. In the former study, Langan et al. [105] prepared the deuterated cellulose II fibers, designated the D-cellulose-II, by mercerization of flax fibers in NaOD/D2O solution. The two neutron diffraction data with 1.2 A˚ resolution were collected from the D-cellulose-II and the ordinary cellulose II fiber or H-cellulose-II. The phasing model of cellulose II was established using the published x-ray diffraction data of Kolpak and Blackwell [86]. As has been observed in the h-D-cellotetraose hemihydrate crystal structures [102,103], the all-gt model is preferred over the gt/tg hybrid model and the D-glucopyranose geometries of the center chain are conformationally strained. The Fourier difference maps calculated from the neutron diffraction data of the D- and H-cellulose II locate the deuterium positions on the phasing models, which reveals details of hydrogen bonding scheme shown in Fig. 24. The two intramolecular hydrogen bonds, O(3)UDUO(5) and O(3)UDUO(6), compose the three-center bond where the former plays the role of the major component in both the origin and center chains. The intermolecular and intrasheet hydrogen bonds are also formed between O(2) and O(6) atoms in both the chain sheets, but they exhibit the opposite donor–acceptor pattern of a deuterium atom. As for the intermolecular and intersheet hydrogen bonds, O(6) of the origin chain donates the deuterium atom to three acceptors of the center chain, forming the four-centered bonding scheme which consists of the O(6)UDUO(6), O(6)UDUO(3), and O(6)UDUO(5) bonds in this strengthening order. Another major bond of this type is the O(2)UDUO(2) bond from the center chain to the origin chain. The following high-resolution synchrotron x-ray diffraction study with 1 A˚ resolution indicated better fitting of the diffraction data to the all-gt model than that of the Kolpack and Blackwell data [106]. The report also suggested that the four-centered hydrogen bond on O(6) of the origin chain is a statistical effect along with the disorder of the hydroxymethyl conformation of the origin chain of which degree is estimated to be about 10%.
REFERENCES 1.
2.
Rees, D.A.; Scott, W.E. Polysaccharide conformation. Pt. VI. Computer model-building for linear and branched pyranoglycans. Correlations with biological function. Preliminary assessment of inter-residue forces in aqueous solution. Further interpretation of optical rotation in terms of chain conformation. J. Chem. Soc. B, 1971; 469. Atkins, E.D.T.; Phelps, C.F.; Sheehan, J.K. The conformation of the mucopolysaccharides, hyaluronates. Biochem. J. 1972, 128, 1255.
120 3. 4. 5. 6. 7.
8. 9. 10.
11.
12.
13.
14.
15.
16.
17.
18. 19. 20. 21. 22. 23.
Yui and Ogawa Ogawa, K.; Misaki, A.; Oka, S.; Okamura, K. X-ray diffraction data for (1!3)-a-D-glucan. Carbohydr. Res. 1979, 75, C13. Marchessault, R.H.; Deslandes, Y.; Ogawa, K.; Sundararajan, P.R. X-ray diffraction data for h-(1!3)-D-glucan. Can. J. Chem. 1977, 55, 300. Millane, R.P.; Arnott, S. Background removal in x-ray diffraction patterns. J. Appl. Crystallogr. 1985, 18, 419. Millane, R.P.; Arnott, S. Digital processing of x-ray diffraction patterns from oriented fibers. J. Macromol. Sci. Phys. 1985, B24, 193. Millane, R.P. Relating reflection boundaries in x-ray fiber diffraction patterns to specimen morphology and their use for intensity measurement. J. Macromol. Sci. Phys. 1989, B28, 149. Okuyama, K.; Obata, Y.; Noguchi, K.; Kusaba, T.; Ito, Y.; Ohno, S. Single helical structure of curdlan triacetate. Biopolymers 1996, 38, 557. Okuyama, K.; Obata, Y. Structure analysis of polybenzamide using imaging plate as x-ray detectors. Polym. Prepr., ACS 1992, 33, 280. Obata, Y.; Okuyama, K. Structural analysis of fibrous polymers by using an imaging plate—A comparison with the conventional photographic method. Kobunshi Ronbunshu (Tokyo) 1992, 49, 297. in Japanese. Obata, Y.; Okuyama, K. Data processing system for x-ray fiber diffraction patterns obtained by using an imaging plate. Kobunshi Ronbunshu (Tokyo) 1994, 51, 297. in Japanese. Smith, P.J.C.; Arnott, S. LALS: A linked-atom leastsquares reciprocal-space refinement system incorporating stereochemical restraints to supplement sparse diffraction data. Acta Crystallogr. 1978, A34, 3. Zugenmaier, P.; Sarko, A. The variable virtual bond modeling technique for solving polymer crystal structures. In Fiber Diffraction Methods; French, A.D., Gardner, K.-C.H., Eds.; ACS Symposium Series, 141; American Chemical Society: Washington, DC, 1980; 225 pp. Millane, R.P.; Narasaiah, T.V. A comparison of the linkedatom squares and PS79 systems for determining polymer structures from x-ray fibre diffraction data. Polymer 1989, 60, 1763. Arnott, S.; Scott, W.E. Accurate x-ray diffraction analysis of fibrous polysaccharide containing pyranose rings. Part I. The linked-atom approach. J. Chem. Soc., Perkin Trans. II 1972; 324. Arnott, S. Twenty years hard labor as a fiber diffractionist. In Fiber Diffraction Methods; French, A.D., Gardner, K.-C.H., Eds.; ACS Symposium Series, 141; American Chemical Society: Washington, DC, 1980; 1 pp. Fraser, R.D.B.; Macrae, T.P.; Suzuki, E. An improved method for calculating the contribution of solvent to the x-ray diffraction pattern of biological molecules. J. Appl. Crystallogr. 1978, 11, 693. Chuah, C.T.; Sarko, A.; Deslandes, Y.; Marchessault, R.H. Triple-helical crystalline structure of curdlan and paramylon. Macromolecules 1983, 16, 1375. Gardner, K.H.; Blackwell, J. Refinement of the structure of h-chitin. Biopolymers 1975, 14, 1581. Minke, R.; Blackwell, J. The structure of a-chitin. J. Mol. Biol. 1978, 120, 167. Roberts, G.A.F. Chitin Chemistry; The Macmillan Press Ltd.: Houndmills, Basingstoke, Hampshire, 1992. Clark, G.L.; Smith, A.F. X-ray diffraction studies of chitin, chitosan, and derivatives. J. Phys. Chem. 1937, 40, 863. Yui, T.; Imada, K.; Okuyama, K.; Obata, Y.; Suzuki, K.; Ogawa, K. Molecular and crystal structure of the anhydrous form of chitosan. Macromolecules 1994, 27, 7601.
24. Sakurai, K.; Shibano, T.; Kimura, K.; Takahashi, T. Crystal structure of chitosan. II. Molecular packing in unit cell of crystal. Sen’i Gakkaishi (Tokyo) 1985, 41, T-361. 25. Ogawa, K. Effect of heating an aqueous suspension of chitosan on the crystallinity and polymorphs. Agric. Biol. Chem., Tokyo 1991, 55, 2375. 26. Okuyama, K.; Noguchi, K.; Miyazawa, T.; Yui, T.; Ogawa, K. Molecular and crystal structure of hydrated chitosan. Macromolecules 1997, 30, 5849. 27. Ogawa, K.; Hirano, S.; Miyanishi, T.; Yui, T.; Watanabe, T. A new polymorph of chitosan. Macromolecules 1984, 17, 973. 28. Cairns, P.; Miles, M.J.; Morris, V.J.; Ridout, M.J.; Brownsey, G.J.; Winter, W.T. X-ray fibre diffraction studies of chitosan and chitosan gels. Carbohydr. Res. 1992, 235, 23. 29. Ogawa, K.; Inukai, S. X-ray diffraction study of sulfuric, nitric, and halogen acid salts of chitosan. Carbohydr. Res. 1984, 160, 425. 30. This notation defines a hydroxymethyl conformation: gg, gauche to C5–O5 and gauche to C4–C5; gt, gauche to C5– O5 and trans to C4–C5; tg, trans to C5–O5 and trans to C4– C5. 31. Kawada, J.; Yui, T.; Okuyama, K.; Ogawa, K. Crystalline behavior of chitosan organic acid salts. Biosci. Biotechnol. Biochem. 2001, 65, 2542. 32. Muzzarelli, R.A.A. Chitin; Pergamon Press: Oxford, 1977. 33. Ogawa, K.; Nakata, K.; Yamamoto, A.; Nitta, Y.; Yui, T. X-ray study of chitosan L- and D-ascorbates. Chem. Mater. 1996, 8, 2349. 34. Yamamoto, A.; Kawada, J.; Yui, T.; Ogawa, K. Conformational behavior of chitosan in the acetate salt. Biosci. Biotechnol. Biochem. 1997, 61, 1230. 35. Kawada, J.; Yui, T.; Abe, Y.; Ogawa, K. Crystalline features of chitosan–L- and D-lactic acid salts. Biosci. Biotechnol. Biochem. 1998, 62, 700. 36. Kawada, J.; Abe, Y.; Yui, T.; Okuyama, K.; Ogawa, K. Crystalline transformation of chitosan from hydrated to anhydrous polymorph via chitosan monocarboxylic acid salts. J. Carbohydr. Chem. 1999, 18, 559. 37. Okuyama, K.; Noguchi, K.; Kanenari, M.; Egawa, T.; Osawa, K.; Ogawa, K. Structural diversity of chitosan and its complexes. Carbohydr. Polym. 2000, 41, 237. 38. Ogawa, K.; Oka, K.; Miyanishi, T.; Hirano, S. X-ray Diffraction Study on Chitosan–Metal Complexes; In Chitin, Chitosan, and Related Enzymes; Zikakis, J.P., Ed.; Academic Press, INC: Orlando, 1984; 327 pp. 39. Ogawa, K.; Oka, K.; Yui, T. X-ray study of chitosan– transition metal complexes. Chem. Mater. 1993, 5, 726. 40. Schlick, S. Binding sites of Cu2+ in chitin and chitosan. An electron spin resonance study. Macromolecules 1986, 19, 192. 41. Takagi, H.; Kadowaki, K. Flocculant production by Paecilomyces sp. taxonomic studies and culture conditions for production. Agric. Biol. Chem., Tokyo 1985, 49, 3151. 42. Takagi, H.; Kadowaki, K. Purification and chemical properties of a flocculant produced by Paecilomyces. Agric. Biol. Chem., Tokyo 1985, 49, 3159. 43. Ogawa, K.; Tanaka, F.; Tamura, J.; Kadowaki, K.; Okamura, K. Structure of a poly[(1!4)-a-D-galactosamine anhydride] studied by x-ray diffraction coupled with conformational analysis. Macromolecules 1987, 20, 1172. 44. Bohn, J.A.; BeMiller, J.N. (1!3)-h-D-Glucans as biological response modifiers: a review of structure–functional activity relationships. Carbohydr. Polym. 1995, 28, 3. 45. Harada, T.; Harada, A. Curdlan and Succinoglycan. In Polysaccharides in Medical Applications; Dumitriu, S., Ed.; Marcel Dekker, Inc.: New York, 1996; 21 pp.
X-ray Diffraction Study of Polysaccharides 46. Deslandes, Y.; Marchessault, R.H.; Sarko, A. Triplehelical structure of (1!3)-h-D-glucan. Macromolecules 1980, 13, 1466. 47. Bluhm, T.L.; Sarko, A. The triple helical structure of lentinan, a linear h-(1!3)-D-glucan. Can. J. Chem. 1977, 55, 293. 48. Kasai, N.; Harada, T. Ultrastructure of curdlan. In Fiber Diffraction Methods; French, A.D., Gardner, K.-C.H., Eds.; ACS Symposium Series, 141; American Chemical Society: Washington, DC, 1980; 363 pp. 49. Fulton, W.S.; Atkins, E.D.T. The gelling mechanism and relationship to molecular structure of microbial polysaccharide curdlan. In Fiber Diffraction Methods; French, A.D., Gardner, K.-C.H., Eds.; ACS Symposium Series, 141; American Chemical Society: Washington, DC, 1980, 385 pp. 50. Okuyama, K.; Otsubo, A.; Fukuzawa, Y.; Ozawa, M.; Harada, T.; Kasai, N. Single-helical structure of native curdlan and its aggregation state. J. Carbohydr. Chem. 1991, 10, 645. 51. Bluhm, T.L.; Deslandes, Y.; Marchessault, R.H.; Perez, S.; Rinaudo, M. Solid-state and solution conformation of scleroglucan. Carbohydr. Res. 1982, 100, 117. 52. Takahashi, Y.; Kobatake, T.; Suzuki, H. Triple helical structure of schizophyllan. Rep. Prog. Polym. Phys. Jpn. 1984, 26, 767. 53. Norisuye, T.; Yanaki, T.; Fujita, H. Triple helix of a Schizophyllum commune polysaccharide in aqueous solution. J. Polym. Sci., Polym. Phys. Ed. 1980, 18, 547. 54. Norisuye, T. Triple-stranded helical structure of schizophyllan and its antitumor activity of aqueous solution. Makromol. Chem., (Suppl.) 1985, 14, 105. 55. Okuyama, K.; Noguchi, K. Structural studies on polysaccharides by using structural information of the related oligosaccharides. Kobunshi (Tokyo) 1994, 43, 848. in Japanese. 56. Noguchi, K.; Kobayashi, E.; Okuyama, K.; Kitamura, S.; Takeo,K.;Ohno,S.(2,3,4,6-tetra-O-acetyl-h-D-Glucopyranosyl)–(1!3)-[2,3,4,6-tetra-O-acetyl-h-D-glucopyranosyl]–(1!6)]-(2,4-di-O-acetyl-h-D-glucopyranosyl)–(1!3)1,2,4,6-tetra-O-acetyl-h-D-glucopyranose. Carbohydr. Res. 1994, 258, 35. 57. Ebisu, S.; Misaki, A.; Kato, K.; Kotani, S. The structure of water-insoluble glucans of cariogenic Streptococcus mutans, formed in the absence and presence of dextranase. Carbohydr. Res. 1974, 38, 374. 58. Tsumuraya, Y.; Misaki, A. Structure of the water-insoluble a-D-glucan of Streptococcus salivarius HHT. Carbohydr. Res. 1979, 74, 217. 59. Ogawa, K.; Okamura, K.; Sarko, A. Molecular and crystal structure of the regenerated form of (1!3)-a-D-glucan. Int. J. Biol. Macromol. 1981, 3, 31. 60. Jelsma, J.; Kreger, D.R. Polymorphism in crystalline (1!3)-a-D-glucan from fungal cell-walls. Carbohydr. Res. 1979, 71, 51. 61. Jelsma, J. Ultrastructure of Glucans in Fungal Cell Walls, Thesis, University of Groningen, 1979. 62. Ogawa, K.; Yui, T.; Okamura, K.; Misaki, A. Crystalline features of streptococcal (1!3)-a-D-glucans of human saliva. Biosci. Biotechnol. Biochem., Tokyo 1994, 58, 1326. 63. Sone, Y.; Kakuta, M.; Misaki, A. Isolation and characterization of polysaccharides of ‘‘Kikurage’’, fruiting body of Auricularia auricula-judae. Agric. Biol. Chem., Tokyo 1978, 42, 417. 64. Kakuta, M.; Sone, Y.; Umeda, T.; Misaki, A. Comparative structural studies on acidic heteropolysaccharides isolated from ‘‘Shirokikurage’’, fruit body of Tremella fuciformis
121
65. 66.
67. 68. 69.
70. 71.
72.
73.
74.
75. 76. 77.
78. 79. 80. 81. 82.
berk, and the growing culture of its yeast-like cells. Agric. Biol. Chem., Tokyo 1979, 43, 1659. Yui, T.; Ogawa, K.; Sarko, A. Molecular and crystal structure of the regenerated form of (1!3)-a-D-mannan. Carbohydr. Res. 1992, 229, 57. Okuyama, K.; Arnott, S.; Moorhouse, R.; Walkinshaw, M.D.; Atkins, E.D.T.; Wolf-Ullish, CH. Fiber diffraction studies of bacterial polysaccharides. In Fiber Diffraction Methods; French, A.D., Gardner, K.-C.H., Eds.; ACS Symposium Series, 141; American Chemical Society: Washington, DC, 1980; 411 pp. Upstill, C.; Atkins, E.D.T.; Attwool, P.T. Helical conformation of gellan gum. Int. J. Biol. Macromol. 1986, 8, 275. Chandrasekaran, R.; Millane, R.P.; Arnott, S.; Atkins, E.D.T. The crystal structure of gellan. Carbohydr. Res. 1988, 175, 1. Chandrasekaran, R.; Thailambal, V.G. A new generation of gel-forming polysaccharides. In Computer Modeling of Carbohydrate Molecules; French, A.D. Brady, J.W., Eds.; ACS Symposium Series, 430; American Chemical Society: Washington, DC, 1990; 300 pp. Kuo, M.-S.; Mort, A.J.; Dell, A. Identification and location of L-glycerate, an unusual acyl substituent in gellan gum. Carbohydr. Res. 1986, 156, 173. Ooiso, Y.; Okumiya, T.; Kawashima, K.; Sone, Y.; Kakuta, M.; Misaki, A. Beijeran, a New Acidic Polysaccharide Produced by Azotobacter beijerinckii YNM1: Structure and Rheological Properties, Abstract of XVIIth Japanese Carbohydrate Symposium, 1995, Kyoto, p. 89. Misaki, A.; Ooiso, Y.; Kakuta, M.; Sone, Y.; Ogawa, K. Structure and Functional Properties of Beijeran, a New Exopolysaccharide of Azotobacter beijerinckii, Abstract of XVII International Carbohydrate Symposium, 1996, Milano, p. 651. Ogawa, K.; Yui, T.; Nakata, K.; Nitta, Y.; Kakuta, M.; Misaki, A. Chain conformation of deacetylated beijeran calcium salt. Biosci. Biotechnol. Biochem., Tokyo 1996, 60, 551. Ogawa, K.; Yui, T.; Nakata, K.; Kakuta, M.; Misaki, A. X-ray study of beijeran sodium salt, a new galacturonic acid-containing exo-polysaccharide. Carbohydr. Res. 1997, 300, 41. Bian, W.; Chandrasekaran, R.; Ogawa, K. X-ray structure analysis of the sodium salt of beijeran. Carbohydr. Res. 2002, 337, 305. Kishida, N.; Okimasu, S.; Kamata, T. Molecular weight and intrinsic viscosity of konjac gluco-mannan. Agric. Biol. Chem., Tokyo 1978, 42, 1645. Kato, K.; Matsuda, K. Studies on the chemical structure of konjac mannan, pt. I. Isolation and characterization of oligosaccharides from the partial acid hydrolyzate of the mannan. Agric. Biol. Chem., Tokyo 1969, 33, 1446. Ogawa, K.; Yui, T.; Mizuno, T. X-ray diffraction study of glucomannans and their acetates. Agric. Biol. Chem., Tokyo 1991, 55, 2015. Yui, T.; Ogawa, K.; Sarko, A. Molecular and crystal structure of konjac glucomannan in the mannan II polymorphic form. Carbohydr. Res. 1992, 229, 41. Chanzy, H.D.; Grosrenaud, A.; Joseleau, J.P.; Dube, M.; Marchessault, R.H. Crystallization behavior of glucomannan. Biopolymers 1982, 21, 301. Meyer, K.H.; Misch, L. Position des Atomes dans le Nouveau Modele Spatial de la Cellulose. Helv. Chim. Acta 1937, 20, 232. Sarko, A.; Muggli, R. Packing analysis of carbohydrates and polysaccharides. III. Valonia cellulose and cellulose II. Macromolecules 1974, 7, 486.
122 83. 84.
85.
86. 87. 88. 89. 90. 91.
92. 93.
94. 95.
Yui and Ogawa Gardner, K.H.; Blackwell, J. The structure of native cellulose. Biopolymers 1974, 13, 1975. Woodcoock, C.; Sarko, A. Packing analysis of carbohydrate and polysaccharides. 11. Molecular and Crystal structure of native ramie cellulose. Macromolecules 1980, 13, 1183. Stipanovic, A.J.; Sarko, A. Packing analysis of carbohydrate and polysaccharides. 6. Molecular and crystal structure of regenerated cellulose II. Macromolecules 1976, 9, 851. Kolpak, F.J.; Blackwell, J. Determination of the structure of cellulose II. Macromolecules 1976, 9, 273. The chain direction is defined as ‘‘up’’ when the z coordinate of O5 is greater than that of C6, and it is defined as ‘‘down’’ otherwise. Honjo, G. Examination of cellulose fiber by the lowtemperature specimen method of electron diffraction and electron microscopy. Nature 1958, 181, 326. Attala, R.; VanderHart, D.L. Native cellulose: a composite of two distinct crystalline forms. Science 1984, 223, 282. VanderHart, D.L.; Attala, R. Studies of microstructures in native cellulose using solid-state 13CNMR. Macromolecules 1984, 17, 1465. Sugiyama, J.; Okano, T.; Yamamoto, H.; Horii, F. Transformation of Valonia cellulose crystals by an alkaline hydrothermal treatment. Macromolecules 1990, 23, 3196. Sugiyama, J.; Persson, J.; Chanzy, H. Combined infrared and electron diffraction study of the polymorphism of native celluloses. Macromolecules 1990, 24, 2461. Sugiyama, J.; Vuong, R.; Chanzy, H. Electron diffraction study on the two crystalline phases occurring in native cellulose form algal cell wall. Macromolecules 1991, 24, 4168. French, A.D.; Miller, D.P.; Aabloo, A. Miniature crystal models of cellulose polymorphs and other carbohydrates. Int. J. Biol. Macromol. 1993, 15, 30. Aabloo, A.; French, A.D. Preliminary potential energy
96. 97. 98. 99. 100.
101.
102.
103.
104. 105.
106.
calculations of cellulose Ia crystal structure. Macromol. Theory Simul. 1994, 3, 185. Aabloo, A.; French, A.D.; Mikesaar, R.; Prestin, A.J. Studies of crystalline native cellulose using potential energy calculations. Cellulose 1994, 1, 161. Heiner, A.P.; Sugiyama, J.; Teleman, O. Crystalline cellulose Ia and Ih studied by molecular dynamics simulation. Carbohydr. Res. 1995, 273, 207. Vie¨tor, R.J.; Mazeau, K.; Lakin, M.; Pe´rez, S. A priori crystal structure prediction of native cellulose. Biopolymers 2000, 54, 342. Finkenstadt, V.L.; Millane, R.P. Crystal structure of Valonia cellulose Ih. Macromolecules 1998, 31, 7776. Nishiyama, Y.; Langan, P.; Chanzy, H. Crystal structure and hydrogen-bonding system in cellulose Ih form synchrotron x-ray and neutron fiber diffraction. J. Am. Chem. Soc. 2002, 124, 9074. Gessler, K.; Krauss, N.; Steiner, T.; Sandman, C.; Betzel, C.; Saeger, W. Crystal structure of b-D-cellotetraose hemihydrate with implications for the structure of cellulose II. Science 1994, 266, 1027. Gessler, K.; Krauss, N.; Steiner, T.; Sandman, C.; Sarko, A.; Saeger, W. h-D-Cellotetraose hemihydrate as a structural model for cellulose II. An x-ray diffraction study. J. Am. Chem. Soc. 1995, 117, 11397. Raymond, S.; Heyraud, A.; Tran Qui, D.; Kvick, A˚.; Chanzy, H. Crystal and molecular structure of h-Dcellotetraose hemihydrate as a model of cellulose II. Macromolecules 1995, 28, 2096. Raymond, S.; Kvick, A˚.; Chanzy, H. The structure of cellulose II: A revisit. Macromolecules 1995, 28, 8422. Langan, P.; Nishiyama, Y.; Chanzy, H. A revised structure and hydrogen-bonding scheme in cellulose II form a neutron fiber diffraction analysis. J. Am. Chem. Soc. 1999, 121, 9940. Langan, P.; Nishiyama, Y.; Chanzy, H. X-ray structure of mercerized cellulose II at 1 A˚ resolution. Biomacromolecules 2001, 2, 410.
5 Recent Developments in Spectroscopic and Chemical Characterization of Cellulose Rajai H. Atalla USDA Forest Service and University of Wisconsin, Madison, Wisconsin, U.S.A.
Akira Isogai Graduate School of Agricultural and Life Science, University of Tokyo, Tokyo, Japan
I. INTRODUCTION
II. STRUCTURES
This chapter represents a summary review and an update of an earlier discussion of the phenomenology of cellulose, together with an overview of recent developments in the chemistry of cellulose. Rather than attempting to integrate the discussions, they will be presented in two separate sections. Part A, by R.H. Atalla, deals with the states of aggregation of celluloses and key structural issues, particularly those with questions of structure still outstanding. Part B, by A. Isogai, presents an overview of recent developments in the chemistry of cellulose, both basic and applied. To minimize the possibility of confusion, the references and figures are numbered consecutively and separately for each of the sections.
The beginning of the last three decades of studies on the structure of cellulose was marked by the reintroduction of unit cell models based on parallel alignment of the cellulose molecular chains [2,3], not unlike those abandoned by Meyer and Misch [4] in the 1930s, but also incorporating bending of the glycosidic linkage to allow the intramolecular hydrogen bond, as suggested by Hermans [5]. The new models were not consistent with each other, however, apart from the fact that both were based on parallel alignment of the cellulose chains. As French [6] pointed out, they were also not strongly preferred over an antiparallel structure. In the analysis by French [6], it was recognized that the source of the inconsistency was not so much that the different laboratories were using different computational approaches as it was that the different diffractometric data sets were gathered from different samples and represented different intensities for the same reflections. All of these studies were undertaken before the variability of the crystalline forms of native celluloses was revealed through the high-resolution solid-state 13C NMR investigations. The new crystallographic models also remained in question because the analyses on which they were based incorporated a level of symmetry in the unit cell that was inconsistent with some of the diffractometeric data. Some of the reflections that are consistently observed in electron diffraction patterns and are disallowed by the selection
Part A Spectroscopic Characterization In Part A, we will be concerned with delineating the frontiers of our understanding of cellulose, particularly with respect to its native forms. The presentation is also relevant to the industrial utilization of cellulose, because it addresses the nature of the native forms of many of the feedstocks used, as well as the effects of processes of isolation on structure and reactivity. The evolution of the historical perspective is included in an earlier report [1] and in references cited therein.
123
124
rules for the space group P21 [3] were ignored in these crystallographic analyses. In addition to the disallowed reflections in the electron diffraction patterns that placed the crystallographic models in question, new spectral evidence was developed pointing to the need for further refinement of the structural models, particularly for native celluloses. The models derived from the crystallographic studies could not rationalize many features of the spectral data known to be quite sensitive to structural variations. On the other hand, electron microscopic studies based on new staining techniques, specific to the reducing end groups of the polysaccharides, confirmed the parallel alignment of molecular chains within the microfibrils in native celluloses. These findings were further confirmed by the manifestation, at the electron microscopic level, of the action of cellulases specific to the nonreducing end group; they were clearly active at only one end of each microfibril. The remaining questions at the time, therefore, were concerned with the degree to which the symmetry of space group P21 is consistent with the other structuresensitive observations. It is well to revisit the issue of levels of structure at this point and clarify the levels at which the different investigative methods are most sensitive. The crystallographic models, which represent coordinates of the atoms in the unit cell, represent the most complete possible specification of structure because they include primary, secondary, and tertiary structures. And indeed, crystallographic studies of the monosaccharides and of related structures provide the basis for considerable information concerning bond lengths and bond angles, as well as conformations in saccharide structures. However, for polymeric systems, the diffractometric data are far more limited than for a single crystal of a low-molecular weight compound, so that diffraction data from a polymer must be complemented by information from other structure-sensitive methods. An acceptable model must rationalize not only the diffractometric data, which for cellulose are quite limited in comparison to the number of coordinates that must be specified in a definition of the unit cell, but it must also be such that they can be reconciled with information derived from other experimental measurements known to be sensitive to different levels of structure. The new spectral evidence that must be rationalized by any acceptable structure came from two methodologies that are most sensitive to structure at the secondary and tertiary levels. These are Raman spectroscopy and solidstate 13C nuclear magnetic resonance (NMR) spectroscopy, both of which were applied to cellulosic samples for the first time during the mid-1970s. The exploration of spectra measurable by these two methods can provide significant information concerning both secondary and tertiary structures in the solid state. Because the spectral features observed are also sensitive to molecular environment, they are influenced by the degree of symmetry of the aggregated state. Hence they provide another avenue for exploration of the applicability of the symmetry of space group P21 to the structures of the solid state.
Atalla and Isogai
III. NEW SPECTROSCOPIC METHODS A. Raman Spectroscopy Both Raman and infrared spectroscopy provide information about chemical functionality, molecular conformation, and hydrogen bonding. Raman spectroscopy, however, has some important advantages in the study of biological materials. The key advantage arises from the different bases for activity of molecular vibrations in the Raman and infrared spectra. That is, whereas activity in the infrared region requires finite transition moments involving the permanent dipoles of the bonds undergoing vibrations, activity in the Raman spectrum requires finite transition moments involving the polarizabilities of the bonds. Thus in infrared spectroscopy, the exchange of energy between the molecules and the exciting field is dependent on the presence of an oscillating permanent dipole. In Raman spectroscopy, in contrast, the exciting field induces a dipole moment in the molecule and the induced moment then becomes the basis for exchange of energy with the exciting field. It is useful in this context to view bonds in terms of Pauling’s classification [7] along a scale between the two extremes of polar and covalent. Bonds that are highly polar and possess relatively high dipole moments and reduced polarizabilities tend, when they undergo vibrational transitions, to result in bands that are intense in the infrared and relatively weak in Raman spectra. Conversely, bonds that are primarily covalent in character and have relatively low permanent dipoles and high polarizabilities generally result in bands that are intense in the Raman spectra, but are relatively weak in the infrared. This is perhaps best illustrated by the fact that O2 and N2, which are homonuclear and without permanent dipoles, have very intense Raman spectra although they are inactive in infrared absorption, while H2O, with a high permanent dipole moment, is a very strong absorber in the infrared but a very weak Raman scatterer. With respect to cellulose, the O–H groups of cellulose and those of adsorbed water are dominant in many of the spectral features in infrared spectra. In contrast, the skeletal C–C bonds and the C–H bonds dominate the Raman spectra. A further simplification in the Raman spectra results from the circumstance that the selection rules forbidding activity of overtone and combination bands are more rigidly adhered to than is the case in infrared spectra so that the bands observed in Raman spectra are usually confined to the fundamental modes of the molecules under investigation [8]. In the context of studies on the structure of cellulose, the key advantage of Raman spectroscopy is the degree of its sensitivity to the skeletal vibrations of the cellulose molecule, with the mode of packing in the lattice having only secondary effects. This sensitivity is a consequence of the reality that most of the skeletal bonds are C–C bonds and C–O bonds, both of which have relatively high polarizabilities and, hence, high Raman scattering coefficients. The minimal contribution of packing effects arises from the low Raman scattering coefficients of the highly polar O–H
Developments in Characterization of Cellulose
groups, which are the functionalities that are most directly involved in intermolecular associations. The result is that intramolecular variations such as changes in internal coordinates have a significantly greater influence on the Raman spectra than do variations in intermolecular associations. Finally and very significantly, as the studies of the celluloses progressed, it became clear that the most dramatic differences between the spectra associated with different states of aggregation of cellulose occurred in the region between 200 and 700 cm 1, which is generally inaccessible with most infrared spectrometers. These considerations were paramount in the first detailed examination and comparison of the Raman spectra of celluloses I and II [9]; the spectra are shown in Fig. 1. It was concluded that the differences between the spectra, particularly in the low-frequency region, could not be accounted for in terms of chains possessing the same conformation, but packed in different ways in the different lattices. As noted earlier, that had become the accepted rationalization of the differences between celluloses I and II, as developed from diffractometric studies of these two most common allomorphs. The analyses of the Raman spectra led to the proposal that two different stable conformations of the cellulose chains occur in the different allomorphs. To establish a basis for assessing the differences between celluloses I and II, Atalla and coworkers undertook an extensive series of studies of model compounds of increasing complexity [10–18]. The model systems investigated included the 1,5-anhydropentitiols, the pentitols and erythritol, the pentoses, the inositols, the hexoses, and the cellobiose. The studies included comprehensive normal coordinate analyses of the molecular vibrations of each of the groups of model compounds based on complementary infrared and Raman spectra. The objective of these analyses was to establish the degree to which the different classes of vibrational motions contribute to the spectral features in the different regions of the spectrum. Such a comprehensive approach was necessary because the skeletal bond systems occurring in the structures of carbohy-
Figure 1 Raman spectra of high-crystallinity celluloses I and II.
125
drates are predominantly made up of C–C and C–O bonds, which possess similar reduced masses and vibrational force constants and, hence, have very similar vibrational frequencies. In consequence, a high degree of coupling occurs between the vibrations, with the result that very few of the vibrational modes are localized within specific bonds or functional groups. Thus, the traditional group frequency approach common in the assignment of infrared and Raman spectra is of very limited use, except in the case of vibrations localized in the bonds of hydrogen atoms bonded to much heavier atoms such as O or C. On the other hand, the normal coordinate analyses allow identification of the degree to which the vibrations of each of the internal coordinates contributes to each of the observed bands. Because the coupling of the vibrations is very sensitive to changes in the bond angles and in the dihedral angles associated with the bonds the vibrations of which are coupled, the normal coordinate analyses allow a detailed and systematic exploration of the effects of differences in skeletal conformations on the bands associated with particular vibrations. With respect to the question concerning the conformations of celluloses I and II, it is useful to first consider some of the pertinent information developed from the normal coordinate analyses, particularly with respect to the classes of molecular motions associated with the different spectral features. The region below 1500 cm 1 was the primary focus of the early exploration because the intense bands clustered at about 2900 cm 1 can be identified with the C–H stretching vibrations and the region beyond 3000 cm 1 is clearly associated with the O–H stretching vibrations. In addition to the C–H and O–H stretching vibrations, the internal deformation of the methylene group on C6 is the only vibration that closely approximates a group or local mode in the usual sense implicit in discussions of assignments of vibrational spectra; the HCH bending vibration usually occurs above 1450 cm 1. In all other bands at frequencies below 1450 cm 1, the normal coordinate analysis indicated that the vibrations are so highly coupled that, in most instances, no single internal coordinate contributes more than 20% of the potential energy change associated with any particular frequency, although in a few instances contributions were as high as 40%. Thus, as noted above, the traditional group frequency approach to assignment of vibrational spectra, which is based on the concept of local modes, is generally not applicable in this region in the spectra of saccharides. Instead, it is necessary to focus on the classes of internal motions that are associated with the different frequency ranges and to interpret the spectra in terms of the influence that variations in the internal coordinates can have on the coupling between different types of vibrational deformations. For analysis of the spectra of celluloses, it is possible to classify the groups of features in the different spectral regions in terms of the types of internal deformations that make their maximum contributions to bands in those regions. The bands between 1200 and 1450 cm 1 are attributable to modes involving considerable coupling
126
between methine bending, methylene rocking and wagging, and COH in-plane bending motions; these are angle bending coordinates involving one bond to a hydrogen atom and the other to a heavy atom. Significant contributions from ring stretching begin below 1200 cm 1 and these modes, together with C–O stretching motions, dominate between 950 and 1150 cm 1. Below 950 cm 1, angle bending coordinates involving heavy atoms only (i.e., CCC, COC, OCC, OCO) begin to contribute, although ring and C–O stretches and the external bending modes of the methylene group may be major components as well. The region between 400 and 700 cm 1 is dominated by the heavy atom bending, both C–O and ring modes, although some ring stretching coordinates still make minor contributions. In some instances O–H outof-plane bending motions may make minor contributions in this region as well. Between 300 and 400 cm 1, the ring torsions make some contributions, and below 300 cm 1, they generally dominate. In addition to the above generalized categorization concerning modes that occur in one or another of the model compound systems used in the normal coordinate analyses, the spectrum of cellulose will have contributions because of modes centered at the glycosidic linkage. Computations based on the cellodextrins indicate that these modes are strongly coupled with modes involving similar coordinates in the adjacent anhydroglucose rings. The contributions of the different classes of internal coordinates to the different bands are presented in greater detail elsewhere [19]. As noted above and shown in Fig. 1, differences between the Raman spectra of celluloses I and II are quite significant particularly in the region of the skeletal bending modes of vibration. In the region above 800 cm 1, the differences are most obvious with respect to the relative intensities of the bands and the broadening of some of the bands upon conversion from cellulose I to cellulose II. In the region below 700 cm 1, in contrast, the main features are quite different in the two spectra; these differences are even more evident in the spectra of single fibers, which will be presented later. In the analyses of the spectra of model compounds, changes of the magnitude indicated in Fig. 1 were exclusively associated with the occurrence of differences in conformations. It seemed very probable therefore that the differences between the spectra of celluloses I and II reflect a change in molecular conformation accompanying the transition from one form to the other. As the basic ring structure is not expected to change [19], it would appear that variations in the dihedral angles at the glycosidic linkages provide the only opportunity for conformational differences. Because of the controversy surrounding similar conclusions based on crystallographic studies carried out in the early 1960s [21,22], a number of experimental and theoretical avenues for validating this interpretation were pursued. The first consideration was whether a multiplicity of stable conformations is consistent with the results of conformational energy calculations that were available at the time [20,23]. In both studies, the potential energy
Atalla and Isogai
surfaces were found to possess multiple minima. When the additional constraint of a repeat length of approximately 0.515 nm per anhydroglucose unit was added, two minima representing both left-handed and right-handed departures from the twofold helix appeared to be likely loci of the stable conformations. It was noted in this context that these two minima were close to the positions of the dihedral angles of the glycosidic linkages in cellobiose and methyl h cellobioside, respectively, as these were determined from crystallographic studies [24,25]. Next, inquiry was made into the degree to which changes in the dihedral angles about the bonds in the glycosidic linkage could influence the modes of vibration responsible for the spectral features in the different regions of the spectra. Two approaches were adopted for this purpose. The first was based on examining the Raman spectra of polysaccharide polymers and oligomers that were known to occur in different conformations. The second was a theoretical one based on an adaptation of the matrix perturbation treatment used by Wilson et al. [26] to discuss the effects of isotopic substitution on infrared and Raman spectra. The polysaccharide systems chosen for investigation were among those most closely related to cellulose in the sense that they are the a-1,4-linked polymers and oligomers of anhydroglucose. They included amylose and two of its cyclic oligomers, with primary emphasis on the latter, the a- and h-Schardinger dextrins, often also known as cyclohexa- and cyclohepta-amylose. The structures of the two oligomers differ in that the values of the dihedral angles about the bonds of the glycosidic linkages have to change to accommodate the different number of monomer units. Comparison of the Raman spectra of the cyclic dextrins showed that the differences between them were quite minor in the regions above 800 cm 1, but they were quite significant in the lower frequency region dominated by the skeletal bending and torsional modes. The differences were similar in kind and distribution to the differences between celluloses I and II. It was also noted that in earlier studies of the Raman spectra of amylose [27], it had been observed that forms Va and Vh, which are very similar in conformation but had different levels of hydration, had almost identical spectra. In contrast, form B, which is known to have a distinctly different helix period, was found to have a spectrum that differs from those of forms Va and Vh in a manner approximating the differences between the two cyclic oligodextrins. Taken together, the observations of the Raman spectra of the amyloses support the interpretation of the differences between the Raman spectra of celluloses I and II as pointing to differences in the chain conformations localized at the glycosidic linkages. In the theoretical analysis, the method of Wilson et al. [26] was adapted to explore the consequences of variations in the dihedral angles about the bonds in the glycosidic linkage; this approach is discussed in greater detail elsewhere [1]. These considerations led to the conclusion that skeletal bending and torsional modes are altered to a greater degree than the skeletal stretching modes when the dihedral angles associated with the glycosidic linkage undergo variations. When translated to spectral features
Developments in Characterization of Cellulose
in the Raman spectra, these observations point to major differences in the low frequency region below 700 cm 1, and minor ones in the fingerprint region between 900 and 1500 cm 1. These are indeed precisely the types of differences observed in comparisons of the spectra of celluloses I and II. One final consideration that was addressed is the possibility that rotations of the primary alcohol group at C6 could account for the spectral differences seen in the spectra of celluloses I and II and in the spectra of the amyloses. The normal coordinate analyses of the hexoses showed that rotations about the C5–C6 bond can result in minor variations in the region below 600 cm 1, but that the major impact of such rotations is expected in the spectral region above 700 cm 1 [16,17]. With all of the above considerations in mind, it became clear that the only plausible rationalization of the differences between the Raman spectra of celluloses I and II had to be based on the possibility that differences between the skeletal conformations were the key. The first effort to rationalize differences in conformation was based on the results of the conformational energy mappings that were available at the time [20,23]. The key points derived from those analyses, which have been confirmed by more recent studies [28,29], were that the two energy minima associated with variations in the dihedral angles of the glycosidic linkage correspond to relatively small left-handed and right-handed departures from glycosidic linkage conformations that are consistent with twofold helical symmetry. The minima also represented values of the dihedral angles that were very similar to those reported for cellobiose and methyl h cellobioside on the basis of crystallographic analyses [24,25]. The relationship between the different conformations is represented in Fig. 2, which was adapted by Atalla [30] from a diagram first presented by Rees and Skerret [20]. It is a w// map
Figure 2 W/U map (– – – – –) loci of structures with constant anhydroglucose repeat periods; (: : : : : :) loci of structures of constant intramolecular hydrogen bond (O–O) distances; ( _____ ) contours of potential energy minima based on nonbonded interactions in cellobiose; W, hmethylcellobiose, n=2, the twofold helix line; n=3 the threefold helix lines; (R) right-handed, (L) left-handed. The Meyer–Misch structure is at W=180, U=0.
127
presenting different categories of information concerning the conformation of the anhydrocellobiose unit as a function of the values of the two dihedral angles about the bonds in the glycosidic linkage. w is defined as the dihedral angle about the bond between C4 and the glycosidic linkage oxygen and / as the dihedral angle about the bond between C1 and the glycosidic linkage oxygen. The parallel lines indicated by n=3(L), 2, and 3(R) represent values of the dihedral angles that are consistent with a lefthanded threefold helical conformation, a twofold helical conformation, and a right-handed threefold helical conformation, respectively; a twofold helical conformation inherently does not have a handedness to it. The dashed contours represent conformations that have the indicated repeat period per anhydroglucose unit; the innermost represents a period of 5.25 A˚ corresponding to 10.5 A˚ per anhydrocellobiose unit. The two dotted lines indicate conformations corresponding to values of 2.5 and 2.8 A˚ for the distance between the two oxygen atoms anchoring the intramolecular hydrogen bond between the C3 hydroxyl group of one anhydroglucose unit and the ring oxygen of the adjacent unit; the values bracket the range wherein hydrogen bonds are regarded as strong. The two domains defined by solid lines on either side of the twofold helix line (n=2) represent the potential energy minima calculated by Rees and Skerret for the different conformations of cellobiose. Finally, the points marked by J and W represent the structures of cellobiose determined by Chu and Jeffries [24] and the structure of methyl h cellobioside determined by Ham and Williams [25]. The key point to be kept in mind in relation to this diagram is that structures along the twofold helix line and with a repeat period of 10.3 A˚ per anhydrocellobiose unit possess an unacceptable degree of overlap between the van der Waals radii of the protons on either side of the glycosidic linkage. Consideration of these issues together with the results of the Raman spectral observations led to exploration of the possibility that small departures from the twofold helix structures may be small enough that the conformation was still approximated by a twofold helix. Some plausible alternatives were explored. One was motivated by the comparisons of the Raman spectra of cellulose II and of cellobiose in the O–H stretching region [30]. The latter showed a single sharp band superimposed on a broader background, and the band was identified with the O–H stretching vibration of the isolated intramolecular hydrogen bond revealed in the crystal structure [24]; it occurs between the hydroxyl group on C3 of the reducing anhydroglucose unit and the ring oxygen of the nonreducing unit. The spectrum of cellulose II revealed two such sharp bands in the same region; similar bands were observed in the spectra of the cello-oligodextrins [18]. As the frequency at which such bands occur is very sensitive to the distance between the oxygen atoms anchoring the hydrogen bond, it appeared that the structure of cellulose II must incorporate intramolecular hydrogen bonds with two distinct values of the O–O distance. This led to the proposal that successive units in the structure are not equivalent, and that, as a consequence, alternating glycosidic linkages have different sets of dihedral angles defining their coor-
128
dinates [30]. Thus, the dimeric anhydrocellobiose was regarded as the repeat unit of physical structure rather than the anhydroglucose unit. These conclusions, based on the Raman spectra in the O–H region, were confirmed when the solid-state 13C NMR spectra became available [31] as splittings were observed in the resonances associated with C1 and C4, which anchor the glycosidic linkage. The occurrence of these splittings is indicative of the presence of nonequivalent glycosidic linkages within the structure; the NMR spectra will be considered in greater detail in a subsequent section. Upon further reflection, it was recognized that when alternating glycosidic linkages are admitted as an option, and when anhydrocellobiose is viewed as the repeat unit of structure, the alternating glycosidic linkages need not have the same sense of departure from the twofold helix. That is, it was now possible to consider structures wherein the nonequivalent glycosidic linkages are alternating lefthanded and right-handed departures from the twofold helix. Such structures would be ribbonlike and could appear to approximate the twofold helix. The proposal incorporating the alternating glycosidic linkage has the advantage that it can be reconciled with much of the diffractometeric data. If the departure from twofold helical symmetry is relatively small, it may account for the weakness of the reflections that are disallowed by the selection rules of space group P21. Based on the considerations outlined, the model that was adopted as a basis for continuing explorations of the spectra of cellulose was based on the proposal that the glycosidic linkages alternated between small left-handed and right-handed departures from the twofold helical conformation. Thus, differences between the conformations of celluloses I and II now had to be understood in terms of differences in the internal organization of the anhydrocellobiose units that were the basic units of structure [32,33]. In search of a rationalization of the changes in the internal organization of the cellobiose unit associated with the transition from cellulose I to cellulose II, Atalla drew on an analogy with the structures of cellobiose and methyl h cellobioside, which are represented in Fig. 3. The methyl h cellobioside, which has values of the dihedral angles corresponding to a right-handed departure from the twofold helix, also has a bifurcated intramolecular hydrogen bond in which the proton from the C3 hydroxyl group appears to be located between the ring oxygen and the primary alcohol oxygen at C6 of the adjacent unit. This bifurcation is in part responsible for the absence of a sharp OH band in the OH region of the spectrum of the methyl h cellobioside. Atalla suggested that such bifurcated intramolecular hydrogen bonds may occur in connection with every other glycosidic linkage in a molecule of native cellulose; these bifurcated hydrogen bonds would be associated with those glycosidic linkages that have values of the dihedral angles representing right-handed departures from the twofold helix in a manner not unlike those in methyl h cellobioside. The action of mercerizing agents was seen as resulting in the disruption of the bifurcated OH bonds, thus, allowing the glycosidic linkages to relax to slightly greater departure from the twofold helix [22,23]. Such an
Atalla and Isogai
Figure 3
Structure of h-cellobiose and h-methylcellobioside.
explanation would also be consistent with the observation that the two HCH bending bands in the Raman spectra of native celluloses collapse into a single band upon mercerization, suggesting a nonequivalence of the two primary alcohol groups in native cellulose and a shift closer to equivalence upon mercerization. It is also consistent with the greater splitting of the resonances associated with C1 and C4 seen in the solid-state 13C NMR spectra of cellulose II to be discussed in the following section. While the evidence supporting this proposal is strong, it is not conclusive and, thus, awaits further confirmation. Atalla also introduced the terms kI and kII to designate the conformations corresponding to celluloses I and II; the term k0 was introduced to describe cellulose in a disordered state [34].
B. Solid-State 13C NMR Spectra and the Two Forms of Native Cellulose Ia and Ih Although applied to cellulose later than Raman spectroscopy, high-resolution solid-state 13C NMR has provided perhaps the most significant new insights regarding the structures of cellulose, particularly in its native state. The development of high-resolution solid-state NMR spectroscopy and its application to polymeric materials grew from complementary application of a number of procedures that had been developed in NMR spectroscopy. The first is proton carbon cross-polarization (CP) that is used to enhance sensitivity to the low abundance 13C nucleus. This was combined with high-power proton decoupling to
Developments in Characterization of Cellulose
Figure 4 13C CP-MAS spectrum of cotton linters. The horizontal bars indicate the spectral ranges of the corresponding carbon sites in the anhydroglucose monomer unit of cellulose.
eliminate the strong dipolar interaction between the 13C nuclei and neighboring protons. Finally, the angular dependence of the chemical shift, or chemical shift anisotropy, is overcome by spinning the sample about an axis at a special angle to the direction of the magnetic field, commonly referred to as the magic angle, the procedure denoted by (MAS). The combined application of these procedures, usually designated by (CP/MAS), results in the acquisition of spectra that contain isotropic chemical shift information analogous to that obtained from liquidstate 13C NMR with proton decoupling. In summary, the most important characteristic of the spectra acquired using the (CP/MAS) 13C NMR technique is that, if they are acquired under optimal conditions, they can have sufficient resolution so that chemically equivalent carbons occurring in magnetically nonequivalent sites can be distinguished. In the present context, the corresponding carbons in different anhydroglucose units would be regarded as chemically equivalent. If they are not also symmetrically equivalent, that is, if they occur in different environments or if the anhydroglucose rings possess different conformations, within the rings, or at the glycosidic linkage, or at the primary alcohol group, the carbons will not have magnetically equivalent environments and will, therefore, result in distinctive resonances in the NMR spectrum. The fundamental challenge in the application of this method is to achieve a level of resolution sufficient to distinguish nonequivalences between chemically equivalent carbons, because the magnetic nonequivalence can result in variations in the chemical shift that are small relative to the shifts determined by the primary chemical bonding pattern. Another important feature of the (CP/MAS) 13C NMR technique is that, for a system such as cellulose, which consists of rather rigid hydrogen-bonded molecules and in which all carbons have directly bonded protons, the relative intensities of the resonances are expected to correspond to the proportion of the particular carbons giving rise to them. Thus, the intensities arising from each of the six carbons in the anhydroglucose ring are expected to be equal. This is an important characteristic that is central to
129
the analysis and interpretation of the information contained within the spectra. The first applications of the new technique to cellulose [31,35] demonstrated resolution of multiple resonances for some of the chemically equivalent carbons in the anhydroglucose units. It became clear that rationalization of the spectra that were observed would provide valuable additional information concerning the structure of the celluloses investigated. The first step in such a rationalization was the assignment of the resonances that appear in the spectra. The assignments, which have been discussed in a number of reports [31,35–40], were based on comparisons with solution spectra of cello-oligosaccharides and of a low-DP cellulose [41]. They are indicated in Fig. 4, which shows a spectrum of cotton linters [42]. Beginning at the upfield part of the spectrum, the region between 60 and 70 ppm is assigned to C6 of the primary alcohol group. The next cluster of resonances, between 70 and 81 ppm, is attributed to C2, C3, and C5, the ring carbons other than those anchoring the glycosidic linkage. The region between 81 and 93 ppm is associated with C4, and that between 102 and 108 ppm with C1, the anomeric carbon. In one of the first reports on the application of the technique to studies of different celluloses, the splittings of the resonances of C4 and C1 in the spectrum of cellulose II (Fig. 5) were regarded as confirmation of the occurrence of nonequivalent glycosidic linkages that had earlier been proposed on the basis of the comparison of the Raman spectra of cellulose II and of cellobiose in the O–H stretching region [31]. These splittings were also observed in the CP/MAS spectra of the cello-oligodextrins, which crystallize in a lattice very similar to that of cellulose II. In that context the splittings were attributed to the occurrence of
Figure 5 CP/MAS 13C spectrum of high-crystallinity cellulose II recorded at relatively low resolution. Chemical shifts are shown in parts per million relative to Me4Si. Assignment of the C-1, C-4, and C-6 resonances are based on pertinent liquid-state spectra.
130
nonequivalent cellulose molecules in the same unit cell [38]. However, such an interpretation leaves open the question as to why the resonances for carbons 2, 3, and 5, do not display similar splittings. If the splittings were indeed due to nonequivalent molecules, it would be anticipated that those carbons nearest to the boundaries of the molecule would be the most affected. The carbons anchoring the glycosidic linkage, that is C1 and C4, are the ones most removed from adjacent molecules, yet they also display the greatest splittings. Interpretation of the spectra of native celluloses presented an even more challenging task. In the spectrum of cotton linters (Fig. 4), the two resonance regions associated with C6 and C4 include sharper resonances overlapping broader upfield wings. After excluding the possibility that the broader wings could arise entirely from molecular mobility [35,36], the wings were attributed to cellulose chains in two categories of environment. The first includes all chains located at the surfaces of cellulose microfibrils, which, because of their occurrence at the boundary, are less constrained with respect to the conformations they can adopt. The surfaces are regarded as regions of limited twodimensional order. The importance of this category of order had earlier been demonstrated in a study of different native celluloses undertaken by Earl and VanderHart [36]. The celluloses had natural fibril diameters varying between 3.5 and 20 nm, and it was shown that the areas of the upfield wings of C4 and C6 declined as the surface-tovolume ratio declined. The second category of environments contributing to the upfield wings is that of chains in regions within which the incoherence of order is not limited to two dimensions. Here, the dispersion of the frequencies at which resonances occur may arise from conformational differences, variations in bond geometries, changes in hydrogen bonding patterns, and nonuniformities in neighboring chain environments. These possibilities arise because in such regions the molecular chains are free to adopt a wider range of conformations than the ordering in a crystal lattice or its boundaries would allow. Although the obvious upfield wings of the C4 and C6 resonances are the most direct evidence for the cellulose chains in less-ordered environments, it is expected that the chains in these environments make similar contributions to the resonance regions associated with the other carbons. In the region of C1, the contribution appears to be primarily underneath the sharper resonances, although a small component appears to extend toward 104 ppm. Similarly, it is expected that the contribution from chains in the lessordered environments underlie the sharper resonances of the C2, C3, and C5 cluster. The relative contributions of the two categories of environment to the intensities of the upfield wings were assessed in a careful analysis of the C4 wing [42]. It was demonstrated that part of the wing could be correlated with the range of the C4 resonance in amorphous cellulose prepared by ball milling. It was therefore assigned to cellulose chains occurring in the second type of environment, that is, domains wherein the incoherence of order is extended in all three dimensions. The other part of the wing was attrib-
Atalla and Isogai
uted to chains at the surfaces of the fibrils and, on the basis of these comparisons, it was concluded that approximately 50% of the wing is contributed by cellulose chains in each of the two types of less-ordered environments described in the preceding paragraph. Although the upfield wing of C4 is the basis of this allocation of intensities, it can be assumed that the relative contributions are similar for the upfield wing of C6 and for the component that appears to underlie the sharper resonances at C1. It is also expected that these domains contribute to the total intensity of the C2, C3, and C5 cluster between 70 and 81 ppm. The sharper resonances in the C6 and C4 regions, centered at 66 and 90 ppm, respectively, each appear to consist of more than one resonance line, although the resolution is not sufficient to distinguish the components well. The C6 resonance seems to include at least two components while the C4 resonance appears to include three closely spaced component lines. These multiplicities were interpreted as arising from carbons in cellulose molecules within the interior of crystalline domains and are therefore taken as evidence of the occurrence of chemically equivalent carbons in different magnetic environments within the crystalline domains. The region between 102 and 108 ppm, attributed to C1, also reveals multiplicity and sharp resonance features. Here, however, the shoulder is very limited. It appears that the resonances associated with the two categories of disordered domains described above lie underneath the sharp resonances associated with the interior of the crystalline domains. It can be concluded that, in most instances, the dispersion of frequencies associated with the disorder is small relative to the shift associated with the character of the anomeric carbon C1, while that is not the case for the shifts associated with C4 and C6. One possible rationalization may be that, because of the anomeric effect, the internal coordinates surrounding C1 are much less flexible within the range of possible conformational variations than are the other internal coordinates. In search of a rationalization of the splittings observed in the sharp resonances, (CP/MAS) 13C NMR spectra of a wide variety of samples of cellulose I were recorded. Some of these are shown in Fig. 6. They include ramie fibers (a), cotton linters (b), hydrocellulose prepared from cotton linters by acid hydrolysis (c), a low-DP regenerated cellulose I (d), cellulose from Acetobacter xylinum (e), and cellulose from the cell wall of Valonia ventricosa (f), an alga. While similar observations were reported in a number of studies [31,32,36–40], their implications with respect to structure were more fully developed in the work of VanderHart and Atalla [42,43], which provides the basis for the following discussion. All of the spectra shown in Fig. 6(A–F) are of celluloses that occur in relatively pure form in their native states and require relatively mild isolation procedures. The most striking feature in these spectra, when viewed together, is the variation in the patterns of the multiplets at C1, C4, and C6. These resonances, which are viewed as arising from chains in the interior of crystalline domains, appear to be unique to the particular celluloses; among the native forms
Developments in Characterization of Cellulose
131
Figure 6 13C CP-MAS spectra of several cellulose I samples: (a) ramie; (b) cotton linters; (c) hydrocellulose from cotton linters; (d) a low-DP regenerated cellulose I; (e) Acetobacter xylinum cellulose; (f ) Valonia renrricosa cellulose. Note the varied fine structure particularly at C-1 and C-4. Signal-to-noise variation due to limited amount of some samples. In that instance more polyethylene was added so the side band intensity increased. No line broadening or resolution enhancement techniques were applied in the acquisition of the spectra (after VanderHart and Atalla).
they appear to be distinctive of the source species. The first attempt to rationalize the spectra was in terms of information that they might provide concerning the unit cell of the structure of cellulose I. However, it soon became obvious that such a rationalization was not possible because the relative intensities within the multiplets were not constant, nor were they in ratios of small whole numbers as would be the case if the same unit cell prevailed throughout the crystalline domains. The conclusion was that the multiplicities were evidence of site heterogeniety within the crystalline domains and that therefore native celluloses must be composites of more than one crystalline form. Further rationalization of the spectra required a careful analysis of the mutliplets at C1, C4, and C6, and the variations of the relative intensities of the lines within each multiplet among the spectra of the different celluloses. In addition to excluding a single crystal form on the basis of the considerations noted above, it was also possible to exclude the possibility of three different forms with each contributing a line to the more complex multiplets. Thus, a decomposition of the spectra on the basis of two distinct crystalline forms was pursued. The results of the decom-
position are shown as spectra (b) and (c) in Fig. 7, and were designated as the Ia and Ih forms of native cellulose; this designation was chosen in order to avoid the possibility of confusion with the IA and IB forms that had earlier been defined in terms of differences in the appearance of the O– H bands in different types of native celluloses [44,45]. Spectrum (A) was acquired from a high-crystallinity sample of cellulose II and is included so as to distinguish the heterogeniety of crystalline forms occuring in the different forms of cellulose I from the long-known polymorphic variation of the crystallinity of cellulose. Spectra b and c in Fig. 7 were in fact derived from appropriate linear combinations of the spectra of the lowDP cellulose I (d) and of the A. xylinum cellulose (e) in Fig. 6. Although they represent the best approximations to the two forms of cellulose postulated, they cannot be regarded as representative of the pure forms as they do not adequately reflect the component of the cellulose at the surfaces of the crystalline domains. Spectrum 7B does have some intensity in the upfield wings of C4 and C6, but spectrum 7C has very little evidence of such wings. There is very little question, however, that the sharp components of
132
Figure 7 Comparison of the 13C CP-MAS spectrum (a) of a low-DP cellulose II sample and the spectra (b) and (c) corresponding, respectively, to the two proposed crystalline forms of cellulose I, namely Ia and Ih. Spectra (b) and (c) were obtained by taking linear combinations of the low-DP and Acetobacter cellulose spectra. Discontinuities in spectra (b) and (c) occur where the polyethylene sidebands would have appeared. The Ia spectrum still contains a significant amount of non-Ia resonances as shown by the visible C-4 and C-6 upfield wings. Multiplicities of the C-1, C-4, and C-6 narrower resonances ought to indicate unit cell inequivalences.
spectra 7B and 7C include the key features in the spectra of the Ia and Ih forms. It is of interest to note here that among the distinct resonances of the Ia form at C1, C4, and C6, only the one at C4 appears to be split, while for the Ih form all three resonances associated with these carbons show splitting, with the one at C1 the most pronounced. In an effort to further validate the proposal that the Ia and Ih forms were the primary constituents of native celluloses, VanderHart and Atalla [46] undertook another extensive study to exclude the possibility that experimental artifacts contributed to the key spectral features assigned to the two forms. A number of possible sources of distinctive spectral features were explored. The first was the question whether surface layers associated with crystalline domains within particular morphological features in the native celluloses could give rise to features other than those of the core crystalline domains. The second was whether variations in the anisotropic bulk magnetic susceptibility
Atalla and Isogai
associated with different morphologies could contribute distinctive spectral features. Exploration of the spectra of higher plant celluloses with different native morphologies revealed very little difference in the essential features of the spectra, even after the samples had been subjected to acid hydrolysis. Furthermore, it was concluded that the Ia component of higher plant celluloses was sufficiently low that some question was raised as to whether it occurs at all in these higher plant celluloses. In this context, it was also concluded that without the Ia component in higher plant celluloses, the lineshapes of the Ih form at C4 could only be reconciled with a unit cell possessing more than four anhydroglucose residues per unit cell. Attention was then directed to analysis of the spectra of algal celluloses, wherein the Ia component is the dominant one. Relaxation experiments confirmed that the essential spectral features identified with the two crystalline forms of cellulose were characteristic of the core crystalline domains; when measurements were conducted such that magnetization of the surface domains was first allowed to undergo relaxation, very little change in the spectral features was observed. The relaxation experiments suggested that domains consisting of both the Ia and Ih forms have equal average proximity to the surface. One possible interpretation of these observations, that the two forms are very intimately mixed, was ruled out at that time on the basis of hydrolysis experiments the results of which are now in question. Two groups of modifying experiments were carried out with the algal celluloses. In the first, the algal celluloses were subjected to severe mechanical action in a Waring blender. In the second, the algal celluloses were subjected to acid hydrolysis, in 4 N HCl for 44 h at 100jC. While the mechanical action resulted in some reduction in the proportion of the Ia form, the acid hydrolysis resulted in a dramatic reduction, sufficient indeed to make the spectra seem like those of the higher plants, except that the resolution of the spectral lines was much enhanced relative to that observed in the spectra of even the purest higher plant celluloses. The samples subjected to hydrolysis, wherein the recovery varied between 12% and 22%, were examined by electron microscopy and shown to have lateral dimensions not unlike those of the original samples. These observations were interpreted to imply that the Ia form is more susceptible to hydrolysis than the Ih form. An earlier study of the effect of hydrolysis, under similar conditions but for only 4 h, had been carried out with cellulose from Rhizoclonium heiroglyphicum with no discernible effect on the spectra [47]. The difference in duration of the hydrolysis may well have been the key factor. Both of these observations and their interpretations had been presented, however, before it was recognized that exposure of celluloses with relatively high contents of the Ia form to elevated temperatures can result in its conversion to the Ih form [48]. When the possibility that the Ia content of the algal cellulose had been converted to the Ih form is taken into account, the results of the relaxation experiments of VanderHart and Atalla cited above can be reinterpreted as indicating
Developments in Characterization of Cellulose
133
standing the differences between them and their relationship to each other within the morphology of native cellulosic tissues. A number of complementary approaches were pursued by different investigators in the search for answers. Some were based on further application of solidstate 13C NMR to the study of different celluloses as well as to celluloses that had been subjected to different modifying treatments. Others were based on application of Raman and infrared spectroscopy to new classes of cellulosic samples. Still, others were based on refinement of electron microscopic and electron diffractometric methods. Results of these investigations will be presented in summary.
A. Raman and Infrared Spectra Figure 8 Alternative candidates for the spectra of cellulose Ia (top) and Ih (bottom) derived from linear combinations of the spectra of Ia-rich Cladophera glomerata, before and after acid hydrolysis, which resulted in a Ih-rich cellulose.
intimate mixing of the Ia and Ih forms within the crystalline domains of the algal celluloses. VanderHart and Atalla also took advantage of the spectra derived from the acid hydrolyzed samples of the algal cellulose to generate more highly resolved representative spectra of the Ia and Ih forms. These are shown in Fig. 8, where it is clear that even in the spectrum representative of the Ia form the upfield wings of the C4 and C6 resonances are reduced to a minimum. With the completion of this study by VanderHart and Atalla, most of the questions about the possibility that the spectral features were the results of artifacts were put to rest, and the hypothesis that all native celluloses belong to one or to a combination of these forms was generally accepted. With the above resolution of the questions concerning the nature of native celluloses in mind, it was possible to classify these celluloses with respect to the relative amounts of the Ia and Ih forms occurring in the celluloses produced by particular species. It emerged in these early studies that the celluloses from more primitive organisms such as V. ventricosa and A. xylinum are predominantly of the Ia form, while those from higher plants such as cotton and ramie are predominantly of the Ih form. As noted earlier, the nomenclature chosen was intended to avoid confusion with the IA and IB forms previously used to classify the celluloses on the basis of their infrared spectra in the OH stretching region. In relation to that classification, the NMR spectra suggest that the IA group has the Ia form as its dominant component, while the IB group is predominantly of the Ih form.
IV. FURTHER STUDIES OF STRUCTURES IN CELLULOSE With the wide acceptance of the proposal of the two crystalline forms (Ia and Ih) came the challenge of under-
The categorization of native celluloses into the IA and IB group by Howsmon and Sisson [44] and Blackwell and Marchessault [45] on the basis of the appearance of the OH stretching region of their infrared spectra suggested that the hydrogen bonding patterns within the crystalline domains may be part of the key to the differences between the two forms of native cellulose. This was, in fact, confirmed in the course of more detailed investigations of the Raman spectra carried out on single oriented fibers of native celluloses [49] and in a comprehensive study of the infrared spectra of a number of celluloses of the two forms [50]. The Raman spectral investigations were part of a broader study directed primarily at rationalizing the bands associated with the skeletal vibrational motions and at exploring the differences between celluloses I and II [49]. They differed from earlier Raman spectral studies in that the spectra were recorded with a Raman microprobe on which individual fibers could be mounted for spectral investigation. With this system, it was also possible to explore the variation of the intensity of the bands as the polarization of the exciting laser beam was rotated relative to the axis of the fibers. The observed spectra are shown in Figs. 9 and 10, each of which includes six spectra. Fig. 9 shows the region between 250 and 1500 cm 1, while Fig. 10 shows the region above 2600 cm 1; the region between 1500 and 2600 cm 1 does not contain any spectral features. The spectra in Figs. 9 and 10 are of native and mercerized ramie fibers and of native V. ventricosa, and they are recorded with both parallel and perpendicular polarization of the exciting laser beam. Those identified as 0j spectra were recorded with the polarization of the electric vector of the exciting laser beam parallel to the direction of the fiber axes, while those identified as 90j spectra were recorded with the polarization of the electric vector of the laser perpendicular to the fiber axes. The ramie fibers are known to have the molecular chains parallel to the fiber axes; the V. ventricosa fibers were prepared by drawing the cell wall so as to align the microfibrils within it. A number of features in the spectra are noteworthy with respect to earlier discussions. The first is a comparison of the spectra of V. ventricosa and ramie. It is clear that, apart from a broadening of the bands in the ramie spectra, because of the smaller lateral dimensions of the
134
Atalla and Isogai
the polarization of the exciting radiation is parallel to the chain direction. The sensitivity of the Raman spectra to the orientation of an intramolecular vibrational motion is also illustrated in the intensity of the methine CH stretching band at about 2889 cm 1. It is most intense with the electric vector of the exciting radiation at 90j to the chain axis, an orientation that is parallel to that of the methine C–H bonds of the pyranose rings. Finally, in light of the discussion of the nonequivalence of adjacent anhydroglucose units and the corresponding nonequivalence of alternating glycosidic linkages, the OH region in the 0j spectrum of the mercerized ramie is of particular interest. It shows the two distinct sharp bands that provide evidence of the presence of isolated nonequivalent intramolecular hydrogen bonds in agreement with the alternating glycosidic linkages along the chain; the hydrogen bonds are oriented parallel to the chain direction. This alternation clearly stands out most distinctly in cellulose II. These distinct bands cannot be attributed to nonequivalent chains as the difference in frequency implies a difference in the O–O distances between the oxygen atoms anchoring the hydrogen bond, as well as
Figure 9 Comparison of the Raman spectra from Valonia, ramie, and mercerized ramie (low-frequency region). Spectra were recorded with the electric vector at both 0j and 90j.
crystalline domains, the spectra are very similar except in the OH stretching region. This was interpreted as evidence that the chain conformations in both the Ia and Ih forms are the same, but that the hydrogen bonding patterns between the chains are different within the two forms. This interpretation is more clearly demonstrated in a comparison of the spectra of V. ventricosa and Halocynthia to be presented below. The second feature worthy of note is the dramatic difference between the spectra of native (cellulose I) and mercerized (cellulose II) ramie fibers, particularly in the low-frequency region, which is inaccessible to most infrared spectrometers. This was taken as further confirmation that the conformations of cellulose I and cellulose II must differ sufficiently to result in significant alteration of the coupling patterns between the internal vibrational modes of the pyranose rings in the molecular chains. It is also interesting, in this connection, to compare the intensities of the band at 1098 cm 1 in the spectra of the two forms of ramie. The band is clearly less intense in the spectrum of the mercerized sample, suggesting that a conformational change, which reduces the coupling of the skeletal motions, has occurred. The 1098-cm 1 band is the strongest skeletal band and it is the most intense feature in the spectrum when
Figure 10 Comparison of the Raman spectra from Valonia, ramie, and mercerized ramie (high-frequency region). Spectra were recorded with the electric vector at both 0j and 90j.
Developments in Characterization of Cellulose
a difference in the dihedral angles w and / of the associated glycosidic linkages. Nonequivalent chains would have different periods in the chain direction if they were to possess twofold helical symmetry. The infrared spectral studies of the Ia and Ih forms were carried out by Sugiyama et al. [50] on a number of different native celluloses of both forms. Furthermore, it included examination of a number of Ia-rich celluloses that were converted to the Ih form through the annealing process first reported by Yamamoto et al. [51]. To complement the infrared spectra, Sugiyama et al. [52] recorded electron diffraction patterns for the samples, which allowed classification of the celluloses through comparison with the diffraction patterns acquired in an earlier electron diffractometeric study to be discussed in greater detail in a subsequent section. The key finding emerging from the examination of the infrared spectra of the different forms was that the only differences noted were in bands clearly associated with the OH group. This was also true of the changes observed upon conversion of the Ia form to the Ih form through annealing. The bands associated with both the differences in native forms and with the effects of transformation were observed in both the O–H stretching region above 3000 cm 1 and the O–H out-of-plane bending region between 650 and 800 cm 1. It was reported that spectra of the Ia form had distinctive bands at 3240 and 750 cm 1, while the spectra of the Ih form had distinctive bands at 3270 and 710 cm 1. Furthermore, it was observed that the band at 3240 cm 1 appears to be polarized parallel to the direction of the fibril orientation while the band at 3270 cm 1 is not polarized. Among the low-frequency bands, the one at 710 cm 1
135
appears to be polarized perpendicular to the fibril direction, while the one at 750 cm 1 is not polarized. It was also observed that upon transformation of the Ia-rich celluloses to the Ih form through annealing, the corresponding bands changed accordingly. The authors concurred with the interpretation of the differences between the two forms suggested by Wiley and Atalla, and concluded that the Iato-Ih transformation primarily corresponded to a rearrangement of the hydrogen bond system within the structures and that the two structures appeared to have very similar conformations. The infrared spectral studies by Sugiyama et al. are particularly interesting because they included the spectra of both Valonia and Halocynthia, the Raman spectra of which have been investigated at high resolution [53]. The Raman spectra of Valonia macrophysa and Halocynthia (tunicate) celluloses obtained by Atalla et al. [53] are shown in Fig. 11. These particular spectra are of interest because V. macrophysa is known to be predominantly the Ia form while Halocynthia is predominantly of the Ih form. Comparison of their spectra can be more rigorous than was possible in the earlier work of Wiley and Atalla [49] because the lateral dimensions of the fibrils of both forms are of the order of 20 nm, with the result that their spectra show equal resolution of the bands in all regions of the spectrum. It is to be noted that their spectra are essentially identical in all of the regions associated with skeletal vibrations of all types as well as regions associated with most of the vibrations involving CH bonds, whether in the bending or stretching regions. Indeed, the primary differences between the two spectra are in the broad complex bands occuring in the OH stretching region, and these differences
Figure 11 Raman spectra of Ia-rich Valonia and Ih-rich Haleynthia celluloses. Because both have fibrils of large lateral dimensions, the spectra of both are well resolved and provide a better basis comparison of the spectra of Ia-rich and Ih-rich celluloses.
136
are not unlike those noted in the earlier Raman spectral studies described above. In addition, the weak band at about 840 cm 1 in the spectrum of V. macrophysa has no corresponding band in the spectrum of Halocynthia; this is the band attributed to the out-of-plane bending vibrations of hydrogen-bonded OH groups. There are also minor differences in the relative intensities of the methylene CH stretches and HCH bending vibrations, but these are the natural consequences of different hydrogen bonding patterns for the hydroxyl group at C6. Comparison of the two spectra reinforces the interpretation presented earlier, on the basis of spectra in Figs. 9 and 10, concluding that the only difference between the Ia and Ih forms is in the pattern of hydrogen bonding. Thus, the Raman spectral comparison of the two forms is entirely consistent with that reported for the infrared spectra of these highly crystalline celluloses. It must be kept in mind, of course, that the bands associated with OH group vibrations are not expected to coincide in the Raman and infrared spectra; because of the different bases for activity in the two different spectral approaches to measurement of vibrational frequencies, Raman active vibrational modes are frequently silent in the infrared and vice versa. This, of course, is true for the skeletal bands as well. In view of the considerable variation observed in the Raman spectra of celluloses as a result of changes in molecular conformations, there can be little question that the spectra in Fig. 11 indicate that the conformations of the cellulose molecules in Valonia and Halocynthia are essentially identical. It is also important to note that the Raman spectra of the celluloses from V. macrophysa and V. ventricosa, both of which have been used in different studies as representatives of the Ia form, are effectively indistinguishable in all regions of the spectra. This is also true of the Raman spectra of celluloses from the algae Cladophera glomerata and Rhizoclonium heirglyphicum, which have also been used in many studies as representative of celluloses that are predominantly of the Ia form. In summary, the Raman and infrared spectral studies undertaken after the discovery of the composite nature of native celluloses point to the conclusion that the only difference between the two forms is in the pattern of hydrogen bonding between chains that possess identical conformations. Yet electron microscopic and electron diffractometric studies, to be described in greater detail in a following section, have led to conclusions that the two forms represent two crystalline phases with different crystal habits [52]. It is therefore important to consider what information may be developed from the vibrational spectra with regard to this question. The key conclusion drawn from the electron diffractometeric data was that the Ia form represents a triclinic phase with one chain per unit cell, while the Ih form represents a monoclinic phase with two chains per unit cell. Furthermore, the symmetry of the monoclinic phase appeared to be that of space group P21. It has been recently recognized [53] that such a proposal is not consistent with the vibrational spectra. While it was not possible to have full confidence in this conclusion based on the earlier
Atalla and Isogai
spectral data because of the differences in the level of resolution between the spectra of ramie and Valonia celluloses, the spectra shown in Fig. 11 are of sufficiently high resolution and sufficiently similar that the comparisons can indeed be made with confidence. The key issue is that when crystal structures possess more than one molecule per unit cell, and the molecules have the same vibrational frequencies, the vibrational modes of the unit cell become degenerate. Under these circumstances, couplings will arise between equivalent modes in the different molecules, and it is generally observed that such couplings result in splittings of the bands associated with key vibrational modes. The type of coupling that is relevant in the case of cellulose is that described as correlation field splitting [54]. This effect arises because, as a result of the coupling, the vibrations of a particular mode in the two molecules will now occur at two frequencies that are different from those of the isolated molecule; one of the two new frequencies will have the modes in the two different molecules in phase with each other, while the other will have the modes out of phase with each other. Such correlation field effects result in doublets with a splitting of 10–15 cm 1 in some modes of crystalline polyethylenes having two chains per unit cell. Because no evidence of such splittings occurs in the Halocynthia spectrum shown in Fig. 11, it must be concluded that the Ih form cannot have more than one molecule per unit cell. Nor can it be suggested that the two molecules in a monoclinic unit cell are nonequivalent and may have modes that are at different frequencies, because the skeletal bands in the Halocynthia spectrum are essentially identical to those in the Valonia spectrum. Furthermore, this similarity was also reported in the infrared spectra observed by Sugiyama et al. (cited earlier). Thus, it is clear that the vibrational spectra, both Raman and infrared, point to the conclusion that both the Ia and Ih forms have only one molecule per unit cell. This conclusion of course raises the question as to why the crystallographic data have been viewed for so long as pointing to a two-chain unit cell with the symmetry of space group P21. This is an issue that is best addressed after the results of the electron diffractometric studies have been described in greater detail.
B. Solid-State
13
C NMR Spectra
It is not surprising that the methodology that first provided the basis for understanding the composite nature of native celluloses in terms of the Ia and Ih duality has continued to be the one most often used for seeking deeper understanding of the differences between native celluloses derived from different biological sources. This has been facilitated by the greater availability of solid-state 13C NMR spectrometer systems and by the relative simplicity of the procedures for acquiring the spectra from cellulosic samples. The studies undertaken on the basis of further examination of the solid-state 13C NMR Spectra of celluloses are in a number of categories. The first group is focused on further examination of the spectra of different native celluloses, in part aided by mathematical procedures for
Developments in Characterization of Cellulose
deconvolution of the spectra or for resolution enhancement. Another group relies on exploring the spectral manifestations of native celluloses that have been modified in different ways. Yet, a third approach is based on investigation of celluloses subjected to different but wellknown procedures for inducing structural transformations in the solid aggregated state of cellulose. The group at the Kyoto University Institute for Chemical Research carried out important studies that were complementary to those undertaken by VanderHart and Atalla [42,43,45]. More recently, a number of other groups have made contributions. As a number of questions concerning the nature of the Ia and Ih forms remain outstanding, it is useful to begin with an overview of the findings of different groups in this respect. These will then make it possible to view results of studies by using other methods in a clearer perspective. The early studies by the Kyoto University group have been well summarized in a report that addresses the key points that were the focus of their investigation [55]. In a careful analysis of the chemical shifts of the C1, C4, and C6 carbons in the (CP/MAS) spectra of monosaccharides and disaccharides for which crystallographic structures were available, Horii et al. recognized a correlation between the chemical shifts and the dihedral angles defined by the bonds associated with these particular carbons. In particular, with respect to C6, they demonstrated a correlation between the chemical shift of the C6 resonance and the value of the dihedral angle v defining the orientation of the OH group at C6 relative to the C4–C5 bond in the pyranose ring. This correlation is of value in the interpretation of the solid-state 13C NMR spectra with respect to structure as well as discussion of the implications of splittings of the C6 resonances observed in some of the spectra. Of even greater interest, in light of the discussions of deviations from twofold screw axis symmetry in some of the structures, it was observed that the chemical shifts of C1 and C4 are correlated with the dihedral angles about the glycosidic linkage. In particular, there was a correlation between the shift of C1 and the dihedral angle / about the C1–O bond, and a correlation between the shift of C4 and the dihedral angle w about the O–C4 bond. As the spectra published in the earliest studies did not have sufficient resolution to reveal the splittings of the resonances of C1 and C4, the possibility of occurrence of nonequivalent glycosidic linkages was not addressed at that time. In addition to the analysis of the correlation between the chemical shifts and the dihedral angles, the Kyoto group investigated the distribution of cellulosic matter between crystalline and noncrystalline domains on the basis of measurements of the relaxation of magnetization associated with the different features of the spectra. By measurement of the values of the spin lattice relaxation times T1(C) associated with the different spectral features, they developed a quantification of the degree of crystallinity in the different celluloses. They also undertook analysis of the lineshapes of the different resonances, particularly that of the C4 resonance. The lineshape analysis was based
137
on deconvolution of the spectral features into combinations of Lorentzian functions centered at the assigned shifts for the particular resonances. It is to be noted that the use of Lorentzian functions, which can be justified at a fundamental level in the case of spectra from molecules in solution, has no basis in any fundamental understanding of the phenomenology of acquisition of the solid-state 13C NMR spectra. However, because deconvolution into Lorentzians has been found to be a useful tool in assessing the spectral features in the spectra of cellulose, its use has continued. The qualifications that must be kept in mind when it is used have recently been addressed by VanderHart and Campbell [56]. In the early studies by Horii et al., all of the upfield wing of the C4 resonance was attributed to molecules in noncrystalline domains. On this basis, the lineshape analysis of the C4 resonance of different native celluloses did not seem consistent with the model proposed by VanderHart and Atalla [42] with respect to the composite nature of native celluloses. In later studies, when Horii et al. took note of the fact that, in the study by VanderHart and Atalla, approximately half of the upfield wing of C4 in the spectra of higher plant celluloses was attributed to the surface molecules of crystalline domains, Horii et al. [57] indicated that their results confirm the proposal of VanderHart and Atalla. It is to be noted that in their early reports in this area, Horii et al. used the designations Ib and Ia to designate the different groups of celluloses in which the Ia and Ih forms were dominant. However, in their more recent studies, they have adopted the Ia and Ih designations that are designed to avoid the confusion with the categories first introduced by Howsmon and Sisson discussed earlier. In pursuit of further understanding of the Ia and Ih duality, Horii et al. explored the effects of transformative treatments on the solid-state 13C NMR spectra. The first group of studies was directed at the effects of annealing, first in saturated steam [48], and later in aqueous alkaline solutions (0.1 N NaOH) selected to avoid hydrolytic decomposition of the cellulose [58,59]. In summary, the key findings were that the celluloses wherein the Ia form is dominant are substantially transformed into the Ih form when conditions are established so as to allow the transformation to be complete. The cellulose representative of the Ia form that was used for these studies was V. macrophysa. The effects of the annealing treatment are demonstrated in Fig. 12, which shows the progression in the degree of conversion as the temperature of treatment is increased. Each of the treatments was for 30 min in the aqueous alkaline solution. These results, of course, point to the susceptibility of the Ia form to conversion to the Ih form, suggesting that the latter is the more stable form. To test this hypothesis, a sample of tunicate cellulose, which had earlier been shown to be of the Ih form by Belton et al. [60], was also annealed in an aqueous alkaline solution at 260jC; it showed little change as a result of the annealing [59]. Additional studies by the Kyoto group relied on the solid-state 13C NMR to explore the effects of different variables on the structure of cellulose [61]. It is in order,
138
Figure 12 50-MHz CP/MAS 13C NMR spectra of Valonia cellulose annealed at different temperatures in 0.1 N NaOH solution: (a) original; (b) 220jC; (c) 240jC; (d) 260jC.
in the present context, to briefly note the results of one study in which celluloses from A. xylinum cultures were investigated. One of the variables explored was the temperature of the culture; it was observed that lower temperatures favored the formation of the Ia form at the expense of the Ih form. This finding raises a fundamental question regarding the possibility that the variation of the balance between the two forms is, in part, an adaptive response to changes in the environment. We follow with a commentary on the manifestations in the solid-state 13C NMR spectra of a broader category of structural changes induced by different treatments known to alter the states of aggregation of cellulose. In selecting the investigations to be noted in our discussion, we will focus on studies that provide insight into the variations of the states of aggregation with the history of particular celluloses, both with respect to source and with respect to processes of isolation and transformation. In 1990, Newman and Hemingson [62] began to combine some additional methods of processing the 13C NMR spectral data with those that had been used previ-
Atalla and Isogai
ously such as the monitoring of the value of T1(C) associated with the different spectral features. While these procedures incorporate a significant degree of empiricism, they have facilitated rationalization of the spectral features of a number of native celluloses and are therefore valuable contributions to the repertoire of methods available for interpreting the 13C NMR spectra of native celluloses. It must be noted, however, that the application of these methods has been complemented in the work of Newman and Hemingson, by a considerable degree of awareness of the complexity of the structures of both native and processed celluloses, so that their application by others needs to be approached with this awareness in mind. This work is described in the publications of Newman et al. [62–67], and has been presented in an overview elsewhere [1]. A different approach to mathematical analysis of the solid state 13C NMR spectra of celluloses was introduced by the group at the Swedish Forest Products Laboratory (STFI) [68]. They took advantage of statistical multivariate data analysis techniques that had been adapted for use with spectroscopic methods. Principal component analysis (PCA) was used to derive a suitable set of subspectra from the CP/MAS spectra of a set of well-characterized cellulosic samples. The relative amounts of the Ia and Ih forms and the crystallinity index for these well-characterized samples were defined in terms of the integrals of specific features in the spectra. These were then used to derive subspectra of the principal components, which in turn were used as the basis for a partial least squares analysis of the experimental spectra. Once the subspectra of the principal components are validated, by relating their features to the known measures of variability, they become the basis for analysis of the spectra of other cellulosic samples that were not included in the initial analysis. Here, again, the interested reader can refer to the original publications [68–71] or the overview presented earlier [1].
C. Electron Microscopic Studies The use of electron microscopy in the study of celluloses, particularly in their native state, has resulted in important advances beginning with investigations that were undertaken at the time of the introduction of the earliest electron microscopes. The early work has been ably reviewed by a number of authors [72,73]. Of particular note among these is the coverage of the subject in the treatise by Preston [74]. The earliest and most significant observations, from a structural perspective, were those by Hieta et al. [75], in which they applied a staining method incorporating a chemistry that requires the presence of reducing end groups. They observed that when whole microfibrils of Valonia were viewed, only one end of each microfibril was stained. This clearly indicated that the molecular chains were parallel as the reducing ends of the cellulose chains occurred together at one end of the fibrils. Had the structure been one with an antiparallel arrangement of cellulose chains, it would have been expected that the reducing end groups would occur with equal frequency at
Developments in Characterization of Cellulose
both ends of the microfibril with the result that both ends would be equally stained. The conclusions of Hieta et al. were independently confirmed by another method introduced by Chanzy and Henrissat [76], wherein the microfibrils were subjected to the action of a cellobiohydrolase that is specific in its action on the nonreducing ends of the cellulose chains. They observed a clear narrowing of the tips of the microfibrils to a triangular form at only one end of each microfibril. In this instance, the action was at the nonreducing ends, but the observations were equally convincing evidence that the chains are aligned in a parallel arrangement in these microfibrils. These early studies were focused on microfibrils from algal celluloses that, because of their larger lateral dimensions, could be more easily visualized in detail. More recently, the technique of specific staining of reducing end groups was adapted for application to cotton microfibrils by Maurer and Fengel [77]. In addition to application of the technique to examination of native cellulose, Maurer and Fengel applied the method to examination of microfibrils of mercerized cellulose (cellulose II), for which they also observed staining at only one end of the microfibrils. This last observation, which indicates a parallel chain structure in cellulose II, is very much in contrast to the crystallographic models that point to an antiparallel structure for this form of cellulose. It reinforces the view that the structure of cellulose II still has many uncertainties associated with it, in spite of the many theoretical analyses that have attempted to rationalize the antiparallel form. In yet another important set of investigations by Sugiyama et al. [78–80], reported at approximately the same time, it was demonstrated that lattice images could be recorded from the microfibrils of V. macrophysa. The first images captured were based on lateral observation of the microfibrils [78,79]. Later, the techniques were refined to allow the acquisition of lattice images of cross sections of microfibrils [80]. The significance of these observations was that it was now possible to demonstrate conclusively that the microfibrils are uniform in formation, and that there is no evidence that they are composed of smaller subunits aggregating together to form the individual microfibrils that are observed in the electron micrographs. Thus, the observations resolved some of the questions that had arisen earlier concerning the interpretation of electron micrographs of native celluloses [74,81]; the findings of Sugiyama et al. were the first direct evidence that the approximately 2020-nm cross sections were not composed of distinguishable smaller subunits. It should be noted, however, that the electron diffraction processes responsible for formation of the lattice images are dominated by the organization of the heavy atoms in the molecular chains and would be insensitive to any nonuniformity in the hydrogen bonding patterns within the interior of the 20 20-nm fibrils. The homogeneity of the microfibrils revealed in the lattice images is an issue that needs to be revisited in the context of discussions of biogenesis, for in each instance, the homogeneous crystalline domains clearly include a much larger number of
139
cellulose chains than could possibly arise from the individual membrane complexes associated with the biogenesis of cellulose. Later studies by Sugiyama et al. were based on electron diffraction and were directed at addressing questions concerning the nature of the differences between the Ia and Ih forms of cellulose. In a landmark study [82], electron diffraction patterns were recorded from V. macrophysa in both its native state, wherein the Ia and Ih forms occur in their natural relative proportions, and after annealing using the process first reported by Yamamoto et al. [51], which converts the Ia form into the Ih form. The native material, which is predominantly the Ia form, was shown to produce a complex electron diffraction pattern similar to that which had earlier led Honjo and Watanabe [83] to propose an eight-chain unit cell. In sharp contrast, the annealed sample, which is essentially all of the Ih form, produced a more simple and symmetric pattern that could be indexed in terms of a two-chain monoclinic unit cell. The observed patterns are shown in Fig. 13. Figure 13(a) shows the diffraction pattern of the native forms, while Fig. 13(b) shows how the diffraction pattern is transformed upon annealing. It is the latter that is identified with the Ih form and which has been interpreted to indicate a monoclinic unit cell. Figure 13(c) and (d) are schematic representations of the spots in the diffraction diagrams (a) and (b) and show more clearly how the diffraction pattern is transformed by annealing; the spots marked with arrows are the ones that disappear upon annealing. Upon separating the diffraction pattern of the Ih form from the original pattern, it was possible to identify the components of the original pattern that could be attributed to the Ia form, and it was found to correspond to a triclinic unit cell. In this first report concerning the differences between the diffraction patterns of the Ia and Ih forms, the positioning of the chains within the monoclinic unit cell associated with the Ih form was left open. Two possibilities were regarded as consistent with the diffraction patterns, the first with the twofold screw axes coincident with the molecular chains, the second with the twofold screw axes between the chains. Both possibilities were consistent with the occurrence of nonequivalent anhydroglucose units. The triclinic unit cell associated with the Ia form was also viewed as consistent with two possibilities: the first, a two-chain unit cell and the second, an eightchain unit cell similar to the one first proposed by Honjo and Watanabe [83]. In a later study by Sugiyama et al. [84], the possibilities were narrowed. It was stated that the monoclinic unit cell corresponding to the Ih form was viewed as one wherein the chains were coincident with the twofold screw axes. It was also indicated that the pattern of the triclinic unit cell corresponding to the Ia form appeared consistent with a unit cell with only one chain per unit cell. In both instances, the rationale for these determinations was not presented. Another interesting group of observations reported in the second electron diffraction study by Sugiyama et al. [84] were interpreted as evidence of the occurrence of the two forms of cellulose in separate domains within the same
140
Atalla and Isogai
Figure 13 Typical electron diffraction patterns of V. macrophysa before (a) and after (b) annealing. In the schematic representations of the patterns, the spots marked with arrows correspond to the reflections that disappear during the annealing treatment (after Sugiyama).
microfibrils. It was reported that the subsets of reflections associated with the two different forms could be separately observed, or in combination along the length of an individual microfibril within domains separated by 50 Am from each other. This set of observations was interpreted to indicate an alternation between the Ia and Ih forms along the length of an individual microfibril. Such an interpretation of course raises questions concerning the processes of biogenesis, particularly because the relative proportions of the two forms of cellulose has been found to be invariant for a particular species as long as the procedures used for isolation of the cellulose do not incorporate exposure to conditions that can result in transformations of the Ia form into the Ih form. The observation of different domains producing different diffraction patterns along the same microfibril can be envisioned as arising in two ways. The first is the possibility that the microfibril that was used to acquire the diffraction patterns had a limited amount of curvature or twist to it so that the angle between the electron beam and the unit cell axes was not constant. This could result in differences of relative intensities of diffraction spots from different planes
and, given the short duration of the exposures, result in an unintended editing of the diffraction patterns. Thus, only those diffraction spots that are intense enough to be observed at a particular angle will be detected, while weaker ones go unseen. For example, if the lattice structure first suggested by Honjo and Watanabe [82] is the true one characteristic of the algal celluloses, diffraction patterns observed at different angles would result in different degrees of enhancement of the different subsets of the total diffraction pattern. This would also be true if the threedimensional organization of the chains is more appropriately viewed as a superlattice. Indeed, it is possible that the lattice structure first proposed by Honjo and Watanabe represents the unit cell of such a supelattice. Such an interpretation of these observations is consistent with earlier observations by Roche and Chanzy [85], wherein an electron microscopic image of microfibrils of algal celluloses was formed by use of a technique based on diffraction contrast. It resulted in images of the algal microfibrils that had alternating dark and bright domains that appeared to be of the order of 50 nm in length. This suggests that the Bragg angle associated with a particular
Developments in Characterization of Cellulose
set of reflections is not likely to be coherently ordered relative to the electron beam in domains that are more than 50 nm in length. Given that the coherence of orientation relative to the electron beam was not found to extend beyond 50 nm, it would appear unlikely that it would remain invariant over a distance of 50 Am. An alternative interpretation of the observation is that the alternation of the Ia and Ih forms is real, as proposed by Sugiyama et al. [84], and it reflects an assembly process that is not yet sufficiently well understood. It has been suggested that mechanical stress can facilitate the transformation of the Ia form into the Ih form and that the formation of the Ih form may arise from mechanical deformations of the fibrils in the course of deposition; as they emerge from the plasma membrane they are required, in most instances, to be bent to be parallel to the plane of the cell wall. If this is indeed the source of the reported alternation of the Ia and Ih forms along the microfibril, it would raise questions concerning the uniqueness of the balance between the Ia and Ih forms that seems to be characteristic of particular species.
V. COMPUTATIONAL MODELING The computational modeling has found particular favor in the analyses of large molecules of biological origin. And, of course, cellulose and its oligomers have attracted some attention in this arena. It is valuable to review briefly some of the efforts directed at advancing the understanding of cellulose because, in addition to providing insights regarding the contributions of different classes of interactions, they illustrate the reality that the results of analyses can often be the consequences of assumptions
141
and premises introduced at the outset, rather than conclusions that can provide definitive answers to questions under exploration. As alluded to earlier, the analysis by Rees and Skerret [20] was one of the first computational efforts to explore the constraints on the freedom of variation inherent in the structure of cellobiose. It relied on a potential function that is focused on van der Waals interactions to establish the degree to which domains within w// space may be excluded by hard sphere overlap. The key finding was that approximately 95% of w// space was indeed excluded from accessibility on the basis of hard sphere overlaps that were unacceptable in the sense that they required particular atoms associated with the region of the glycosidic linkage to be significantly closer to each other than the sum of the van der Waals radii. And upon mapping the energy associated with allowable conformations, they found that the two regions indicated by the solid line contours in Fig. 2 represented energy minima close to the conformations defined by the twofold helical constraint. The boundaries of the acceptable region are not very far removed from the domains within the contours; the region between the two domains along the twofold helix line (n=2) was not excluded by hard sphere overlap, but it did represent a saddle point in the potential energy surface. The next group of computational studies did incorporate hydrogen-bonding energies as well the van der Waals interactions. Whether they exhibited the double minima, and the degree to which the double minima were pronounced, depended in large measure on the relative weighting given to the different types of nonbonded interactions. In many, particularly those relying on the potential energy functions incorporated in the linked atom least squares (LALS) programs, the weighting was
Figure 14 Perspective drawing of the three-dimensional shape of the mirror image of the conformational energy well for the full angular range of U and W. The volume was constructed using the following scheme: V(U,W)? 15 kcal 1 mol 1; Vp(U,W)? 1/5 kcal 1; Vp(U,W)= (V(U,W) 15), with V being the energy expressed relative to the minimum. Proceeding from top to bottom of the three-dimensional shape, note the very low energy region (the arrows point towards the conformations observed for crystalline cellobiose and methyl-h-D-cellobioside). The 5–10 kcal 1 mol 1 energy contours correspond to the light gray region of the volume.
142
based on fitting the potential functions to optimize the match between computed structures for small molecules for which the crystal structures were known from crystallographic studies. The results were that some showed very shallow minima off the twofold helix line [23]; the twofold helical structures were then rationalized on the basis that the departure represented a small difference in the energies that were regarded as within the error of the computation. When the criterion for quality of fit is chosen as a global minimum of the potential energy, without attention to the fact that it may incorporate unacceptable hard sphere overlaps, the results of the computational analysis can be misleading. Later studies did not incorporate disproportionate weighting of the different types of nonbonded interactions [28,29], and the result is perhaps best illustrated in the mapping of the potential energy for cellobiose shown in Fig. 14 taken from the study of cello-oligomers by Henrissat et al. [29]. In this instance, for purposes of visualization, the w// map presents the mirror image of the potential energy surface computed for cellobiose. While well more than two minima are shown in this mapping, it is to be noted that only the two corresponding to the crystal structures of cellobiose and methyl-h-cellobioside, marked by arrows, are within the boundaries established in the analysis by Rees and Skerret described earlier. The other minima correspond to conformations that are more favorable to hydrogen bonding, but with relatively high energies associated with the van der Waals interactions pointing to severe hard sphere overlap.
VI. POLYMORPHY IN CELLULOSE One of the discoveries growing out of the early diffractometric studies of cellulose was that it can occur in a number of allomorphic forms in the solid state, each producing distinctive X-ray diffractometric patterns [86]. In addition to the cellulose II form, which has been extensively discussed, two other forms are well recognized: cellulose III and cellulose IV. It is of interest to consider them briefly because they reflect the capacity of cellulose to aggregate in a wide variety of secondary and tertiary structures, and because some of the higher plant celluloses produce diffraction patterns that are not unlike those of cellulose IV. Furthermore, they reflect the tendency for some of the celluloses to retain some memory of their earlier states of aggregation in a manner not yet understood. Cellulose III is of little interest from a biological perspective except to the extent that its behavior may reveal some of the interesting characteristics of the native celluloses from which it can be prepared. It can be prepared from either native cellulose or from cellulose II by treatment with anhydrous liquid ammonia at temperatures near 30jC. It produces distinctive X-ray patterns, Raman spectra, and solid-state 13C NMR spectra. Its most interesting characteristic is that it can be restored to the original form by treatment in boiling water. Because of this characteristic, it is common to designate samples of cellulose III
Atalla and Isogai
as either IIII or IIIII to indicate both the source material and the form that will be recovered if the cellulose is boiled in water. In the case of native celluloses, the transformation to the IIII form and back to the I form, also has the unusual effect of converting those which have the Ia form dominant, such as those from algal sources, into forms in which the Ih form is dominant. This effect, first reported by Chanzy et al. [87], is accompanied by the partitioning of the algal microfibrils into smaller ones that are closer in lateral dimensions to those characteristic of higher plants. The solid-state 13C NMR spectra also then appear more like those of the higher plants. No such changes have been reported for native celluloses in which the Ih form is dominant. These behaviors by cellulose III point to a memory effect with respect to the secondary and tertiary structures of cellulose that remains very much a mystery at the present time. Cellulose IV is most often described as the hightemperature cellulose because it can be prepared by exposing the source cellulose to temperatures in the vicinity of 260jC while it is immersed in glycerol. In this preparation, it is reported to depend in structure on whether it is prepared from cellulose I or cellulose II; hence the frequent designation as IVI or IVII. When prepared from cellulose I, it is first converted to the IIII form prior to the treatment at high temperature in glycerol. When prepared from cellulose II, it can be directly produced from the II form or via the IIIII form as an intermediate. However, in the case of cellulose IV, there are no known procedures that allow restoration to the original form; the use of the different designations reflects some differences in the diffraction patterns observed from the two different forms. Furthermore, most of its reported preparations from native forms of cellulose have been from higher plant celluloses wherein the Ih form is dominant and the lateral dimensions of the native microfibrils are quite small; it is not at all clear that treatment of microfibrils of larger lateral dimensions such as those of Valonia or those of Halocynthia will result in such changes. In addition to its preparation by heating at 260jC in glycerol, cellulose IV has been recovered when cellulose is regenerated from solution at elevated temperatures. This has been observed with solutions in phosphoric acid regenerated in boiling water or in ethylene glycol or glycerol at temperatures above 100jC [88]. It has also been observed upon regeneration from the dimethylsulfoxide–paraformaldehyde solvent system at the elevated temperatures [88]. In yet another exploration of high temperature effects on the aggregation of cellulose, it was found that when amorphous celluloses are prepared under anhydrous conditions and then induced to crystallize by exposure to water, the exposure at elevated temperatures resulted in the formation of cellulose IV rather than cellulose II, which is the form usually obtained upon crystallization at room temperature [89]. Samples of cellulose IV obtained through regeneration from solution were shown to have Raman spectra that could be represented as linear combinations of the spectra of celluloses I and II, suggesting that it may be a mixed
Developments in Characterization of Cellulose
lattice in which molecules with two different secondary structures coexist. This possibility is consistent with the earlier conclusion that both cellulose I and cellulose II have ribbonlike structures that depart, to a limited degree, from a twofold helix but in different ways. It is not at all implausible that molecules so similar in shape could coexist in the same lattice. One of the complications in interpreting observations of the occurrence of cellulose IV is that its X-ray diffraction powder pattern is very similar to that of cellulose I. The 020 reflection is nearly identical to that of cellulose I and the 110 and the 1–10 reflections collapse into a single reflection approximately midway between those of cellulose I. As a result, many of the less well-ordered native celluloses produce X-ray patterns that could equally well be interpreted as indicating cellulose I, but with inadequate resolution of the 110 and 1–10 reflections, or as cellulose IV. They are usually characterized as indicating cellulose I because they represent celluloses derived from native sources. Indeed, when cellulose IV was first observed, it was thought to be a less-ordered form of cellulose I. The close relationship between cellulose IV and the native state is also reflected in reports of its observation in the native state of primary cell wall celluloses. These were observations based on electron diffraction studies of isolated primary cell wall celluloses [90].
VII. CHEMICAL IMPLICATIONS OF STRUCTURE It was noted earlier that an acceptable fit to the diffractometric data is not the ultimate objective of structural studies. Rather, it is the development of a model that possesses a significant measure of validity and usefulness as the basis for organizing, explaining, and predicting the results of experimental observations. In the sections above, the new and evolving conceptual framework for describing the structures of cellulose was described in relation to spectral observations. It is important also to consider the degree to which the structural information that has been developed above may be useful as the basis for advancing the understanding the response of celluloses to chemical reagents and to enzyme systems. It is useful first to review briefly past works directed at rationalizing the responses to such agents. The vast majority of studies of the chemistry of cellulose have been directed at the preparation of cellulose derivatives with varying degrees of substitution depending on the desired product. Sometimes the goal is to prepare a cellulose derivative that possesses properties that significantly differ from those of the native form; some derivatives are water-soluble, others are thermoplastic, and others still are used as intermediates in processes for the regeneration of cellulose in the form of films or fibers. At other times, the objective is to introduce relatively small amounts of substitution to modify the properties of the cellulosic substrate without it losing its macroscopic identity or form such as fiber or microcrystalline powder or regenerated filament or film. All such modification pro-
143
cesses begin with a heterogeneous reaction system, which may or may not eventually evolve into a homogeneous system as the reaction progresses. Thus, in all chemical investigations that begin with cellulose as one of the ingredients, issues associated with heterogeneous reaction systems arise. Understandably, the one that has been dominant in most investigations is the question of the accessibility of the cellulose. A variety of methods have been developed to relate accessibility to microstructure. Almost all of them begin with the premise that the cellulose can be regarded as having a crystalline fraction and a disordered or amorphous fraction. It is then assumed that the amorphous or disordered fraction is accessible while the crystalline fraction is not. In some instances, the portion of the crystalline domains that is at their surface is regarded as accessible and it is therefore included as part of the disordered fraction. In other instances, the particular chemistry is thought to occur only in the disordered fraction and the surfaces of crystalline domains are not included. The different approaches have been reviewed by Bertoniere and Zeronian [91], who regard the different approaches as alternative methods for measuring the degree of crystallinity or the crystalline fraction in the particular celluloses. A number of different chemical and physical approaches are described by Bertoniere and Zeronian. The first is based on acid hydrolysis acids followed by quantification of the weight loss due to dissolution of glucose, cellobiose, and the soluble oligomers [92]. This method is thought to incorporate some error in the quantification of the crystalline domains because the chain cleavage upon hydrolysis can facilitate crystallization of chain molecules that had been kept in disorder as a result of entanglement with other molecules. Another method is based on monitoring the degree of formylation of cellulose when reacted with formic acid to form the ester [93]. In this method, the progress of the reaction with cellulose is compared with a similar reaction with starch, which provides a measure of the possibility of formylation in a homogeneous system wherein the issue of accessibility does not arise. In another method developed by Rowland and his coworkers [94–97], accessible hydroxyl groups are tagged through reaction of the particular cellulose with N,Ndiethylaziridinium chloride to a produce diethylamineether (DEAE)–cellulose. This is then hydrolyzed, subjected to enzyme action to remove the untagged glucose, silylated, and subjected to chromatographic analysis. This method has the added advantage that it can be used to explore the relative reactivity of the different hydroxyl groups. It is usually observed that the secondary hydroxyl group on C2 is the most reactive and the one at C3, the least reactive, with the primary hydroxyl at C6 having a reactivity approaching that of the group on C2 under some conditions. Here, of course, steric effects are also factors in these substitution reactions. Among the physical methods discussed by Bertoniere and Zeronian [91] are ones based on sorption and on solvent exclusion. One of the earliest studies relying on the use of sorption as a measure of accessibility was the
144
classical study by Mann and Marrinan [98], in which deuterium exchange with the protons was monitored. The cellulose was exposed to D2O vapor for a period sufficient to attain equilibrium and then the degree of exchange was measured by observation of the infrared spectra. Comparison of the band associated with the OD stretching vibration with those associated with the OH stretching vibration provided the measure of the relative amounts of accessible and inaccessible hydroxyl groups. Another approach to monitoring availability to adsorbed molecules is measurement of moisture regain upon conditioning under well-defined conditions as described by Zeronian and coworkers [99]. The method of solvent exclusion has been used to explore issues of accessibility on a somewhat larger scale. An approach pioneered by Stone and Scallan [100] and Stone et al. [101] relied on static measurement using a series of oligomeric sugars and dextrans of increasing size to establish the distribution of pore sizes in different preparations of a variety of native celluloses. While methods for characterizing celluloses on the basis of their accessibility have been useful, they do not provide a basis for understanding the level of structure at which the response of a particular cellulose is determined. This follows from the rather simple categorization of the substrate cellulose into ordered and disordered fractions corresponding to the fractions thought to be crystalline and those that are not. This classification does not allow discrimination between effects that have their origin at the level of secondary structure and those that arise from the nature of the tertiary structure. Thus, in terms of chemical reactions, this approach does not facilitate separation of steric effects that follow from the conformation of the molecule as it is approached by a reacting species, from effects of accessibility, which is inherently a consequence of the tertiary structure. The possibility of advancing the understanding of the chemical implications of structure is best illustrated in the context of hydrolytic reactions. Among the patterns that emerge fairly early in any examination of the published literature on acid hydrolysis and on enzymatic degradation of cellulose are the many similarities in the response to the two classes of hydrolytic agents. In both instances, a rapid initial conversion to glucose and cellodextrins is followed by a period of relatively slower conversion, the rate of conversion in the second period depending on the prior history of the cellulosic substrate. In general, the nonnative polymorphic forms are degraded more rapidly during this second phase. In addition, it is found that the most crystalline or highly ordered of the native celluloses are particularly resistant to attack, with the most highly crystalline regions converted much more slowly than any of the other forms of cellulose. The relationship of the patterns of hydrolytic susceptibility to the range of conformational variation discussed above can be interpreted in terms of contrast between the states of the glycosidic linkage in cellobiose and h-methylcellobioside. The differences between the states that are likely to contribute to the differences in observed reactivity
Atalla and Isogai
are of two types. The first is differences in the steric environment of the glycosidic linkage, particularly with respect to activity of the C6 group as a steric hindrance to, or as a potential promoter of, proton transfer reactions, depending on its orientation relative to the adjacent glycosidic linkage. The second type of difference is electronic in nature and involves readjustment of the hybridization of the bonding orbitals at the oxygen in the linkage. It is worthwhile to examine the potential contribution of each of these effects. The steric environment emerges most simply from examination of scale models of the cellodextrins. They reveal that when C6 is positioned in a manner approximating the structure in h-methylcellobioside, the methylene hydrogens are so disposed that they significantly contribute to the creation of a hydrophobic protective environment for the adjacent glycosidic linkage. If, however, rotation about the C5–C6 bond is allowed, the primary hydroxyl group can come into proximity with the linkage and provide a potential path for more rapid proton transfer. If, as suggested earlier on the basis of spectral data, the orientation of some C6 groups in native cellulose is locked in by its participation in a bifurcated hydrogen bond to the hydroxyl group on C3, it may contribute to the higher degree of resistance to hydrolytic action. Access to the linkage oxygen would be through a relatively narrow solid angle, barely large enough to permit entry of the hydronium ions that are the primary carriers of protons in acidic media [102]. If, on the other hand, the C6 group has greater freedom to rotate, as is likely to be the case in cellulose II, the hindrance due to the methylene hydrogens can be reduced and, in some orientations, the oxygen of the primary hydroxyl group may provide a tunneling path for transfer of protons from hydronium ions to the glycosidic linkage. This would result in greater susceptibility of nonnative celluloses to hydrolytic attack. The hypothesis concerning steric effects in acid hydrolysis has as its corollary the proposal that the role of the C1 component in cellulase enzyme system complexes is to disrupt the engagement of the C6 oxygen in the bifurcated intramolecular hydrogen bond and thus permit rotation of the C6 group into a position more favorable to hydrolytic attack. The key role of C6 in stabilizing the native cellulose structures is supported by findings concerning the mechanism of action of the dimethylsulfoxide–paraformaldehyde solvent system for cellulose, which is quite effective in solubilizing even the most crystalline of celluloses. The crucial step in the mechanism that has been established for this system is substitution of a methylol group on the primary hydroxyl at the C6 carbon [103,104]. The effect of conformation on the electronic structure of the linkage is also likely to be a factor with respect to its susceptibility to hydrolytic attack. Although there is no basis for anticipating the directions of this effect at this time, it is well to consider it from a qualitative perspective. First, it is clear that the hybrids of oxygen orbitals involved in the bonds to carbon must be nonequivalent because the bond distances differ to a significant degree [24,25]. The
Developments in Characterization of Cellulose
angle of approximately 116j imposed on the linkage is likely to result in greater differences between the bonding orbitals and the lone pair orbitals than might be expected in a typical glycosidic linkage that is free from strain. Among themselves, the lone pair orbitals are likely to be different because of their different disposition with respect to the ring oxygen adjacent to C1 in the linkage; the differences may be small and subtle, but they are no less real. Given these many influences on the nature of the hybridization at the oxygen in the linkage, it seems most unlikely that they would remain unaltered by changes in the dihedral angles of the magnitude of the difference between cellobiose and h-methylcellobioside. Hence a difference in electronic character must be expected. At present, it is not possible to estimate the magnitude of the effects discussed nor to speculate concerning the direction of the change in relative reactivity of the glycosidic linkage in the two different conformations. Yet it is clear that differences can be anticipated and they may be viewed, within limits of course, as altering the chemical identity of the glycosidic linkage as its conformation changes. It remains for future studies to define the differences more precisely. The points raised with regard to the influence of conformation on factors that determine the pathways for chemical reaction have not been specific subjects of investigation because methods for characterizing secondary structure as apart from the tertiary structure have not been available. It has also been true that suitable conceptual frameworks have not been available for developing the questions beyond the levels of the order–disorder duality. With the development of the approaches outlined above for exploring and distinguishing between matters of secondary structure and those of tertiary structure it is quite likely that in the years ahead, it will be possible to achieve a higher level of organization of information concerning the chemistry of cellulose. With respect to questions of tertiary structure, the key issue introduced by the new structural information, and one that has not been explored at all at this time, is whether the different hydrogen bonding patterns associated with the Ia/Ih duality have associated with the differences between the reactivity of the hydroxyl groups involved. It is not clear at this time how experiments exploring such effects might be carried out so as to separate issues associated with the differences between the hydrogen bonding patterns from issues associated with differences in accessibility.
VIII. CELLULOSE STRUCTURES IN SUMMARY From crystallographic studies, based on both X-ray and electron diffraction measurements, it can be concluded that the secondary structures of native celluloses are ribbonlike conformations approximating twofold helical structures. Their organization into crystallographic unit cells remains uncertain, however. The monoclinic space group P21, with two chains per unit cell, has been proposed for both the earlier studies prior to the discovery of the Ia/Ih duality in
145
native forms, and more recently for the Ih form. The Ia form is thought to possess a triclinic unit cell structure. Some important questions remain regarding the degree to which these are adequate representations of the organization of the crystalline domains in native celluloses. The majority of crystallographic studies also point to parallel alignment of the cellulose chains in the native celluloses, and this conclusion has been confirmed by electron micrographic observations. Also, for cellulose II, the structures derived from the X-ray diffraction data suggest a ribbonlike secondary structure approximating twofold helical organization and, in this instance, antiparallel alignment of the chains, although the antiparallel proposal has been contradicted by recent electron micrographic observations. The unit cell organization of space group P21, with two chains per unit cell, has also been suggested for cellulose II, although the degree of confidence is even less than that with respect to the structures of cellulose I. The early Raman spectroscopic studies clearly could not be reconciled with the premise that both cellulose I and cellulose II possess twofold helical conformations as the crystallographic studies had suggested. The Raman spectra, together with some corresponding infrared spectra, also pointed to the probability that the repeat unit of the structure of crystalline celluloses is anhydrocellobiose, so that alternating nonequivalent glycosidic linkages occur within each chain. To preserve the ribbonlike structural approximation, the different conformations of celluloses I and II were rationalized as alternate left- and right-handed departures from the twofold helical structure, with those in cellulose II representing somewhat larger departures from the twofold helical conformation than those in cellulose I. The introduction of high-resolution solid-state 13C NMR spectral analyses into the study of celluloses resulted in the resolution of one of the fundamental mysteries in the variability of native celluloses by establishing that all native celluloses are composites of two forms. These were identified as the Ia and Ih forms to distinguish them from the IA and IB categories that had been introduced more than three decades earlier to classify the celluloses produced by algae and bacteria from those produced by higher plants. The correspondence between the two classifications is that those in the IA category have the Ia from as the dominant component, while those in the IB category are predominantly of the Ih form. The nature of the difference between the Ia and Ih forms remains the subject of serious inquiry. Recognition of the Ia/Ih duality has facilitated a significant amount of additional research seeking to establish the balance between the two forms in a wide range of higher plant celluloses. In later studies, the Raman spectra and corresponding infrared spectra indicated that the primary differences between the Ia and Ih forms of native cellulose were in the pattern of hydrogen bonding. Furthermore, the Raman spectra of the two forms raise questions as to whether the structures can possess more than one molecule per unit cell because there is no evidence of any correlation field splittings of any of the bands in the spectra of the two forms.
146
Atalla and Isogai
Electron microscopic studies relying on agents that act selectively either at the reducing or at the nonreducing end groups of the cellulose chains have provided convincing evidence that cellulose chains are aligned parallel to one another in native cellulose. More recently, similar evidence has been presented supporting the view that the alignment of the chains is also parallel in cellulose II. Other electron microscopic studies using the methods of lattice imaging have been used to demonstrate that the highly ordered microfibrils derived from algal celluloses represent homogeneous lattice structures with respect to the diffraction planes defined by the organization of their heavy atoms. Electron diffraction studies carried out on algal celluloses after the discovery of the Ia/Ih duality have been interpreted to indicate that the two forms may alternate along the length of individual microfibrils. These observations can also be interpreted as manifestations of the slow twisting about the long axis that has been observed in other studies of similar algal celluloses. The possibility of the coexistence of the Ia and Ih forms within a superlattice structure has been suggested in the context of studies intended to mimic the conditions of biogenesis. These will be examined in greater detail in relation to the discussions of native celluloses and of their biogenesis. Our discussion of structure has focused so far on issues of structure at the nanoscale level, identified as corresponding to domains that are of the order of 2 nm in dimension. Organization at the microscale level, defined as the range between 2 and 50 nm, requires consideration of a number of issues that have not been adequately dealt with in the literature on structures of cellulose. These include the well-recognized departures from a linear lattice, which
Figure 15
have been generally regarded as measures of disorder when, in fact, they are more appropriately regarded as indicators of the nonlinear organization in a biological structure. Another issue arising at the microscale is associated with the occurrence of significant fractions of the cellulose molecules at the surface of the microfibrils of most native celluloses, particularly in the case of higher plants. It is the question as to whether the microfibrillar structure can be viewed as a separate phase in the traditional sense and whether criteria developed for the stability of homogeneous phases in the context of classical thermodynamics can have meaning when applied to native cellulosic structures. These issues arise in relation to discussions of native celluloses and their biogenesis.
Part B Chemical Characterization I. INTRODUCTION Cellulosic materials have been used in various fields from commodities to industrial materials after mechanical and chemical modifications. Fig. 15 illustrates the chemical structure of cellulose in terms of chemical modifications [105]. The h-1,4-glycoside bonds and other functional groups such as carboxyls and aldehydes present in most cellulosic material as minor groups are also possible sites for chemical modifications.
II. SOLVENTS Table 1 summarizes the representative solvents or solvent systems of cellulose. The xanthate system has been used for
Positions in cellulose structure for chemical reactions.
Developments in Characterization of Cellulose
147
Table 1 Conventional and New Cellulose Solvent Systems Category Acid Alkali Alkaline metal system complex
Alkaline xanthogenate derivatives Inorganic salt Organic solvent systems
Solvent
Remarks
>52% H2SO4 >85% H3PO4 6% LiOH 6–9% NaOH Cu(NH3)4(OH)2 [cuoxam] Cu(H2NCH2CH2NH2)2(OH)2 [cuen] Co(H2NCH2CH2NH2)2(OH)2 Ni(NH3)6(OH)2 Cd(H2NCH2CH2NH2)3(OH)2 [cadoxen] Zn(H2NCH2CH2NH2)3(OH)2 Fe/3(tartaric acid)/3NaOH [EWNN] CS2/NaOH
Partial hydrolysis Partial hydrolysis Needs pretreatments of cellulose Needs pretreatments of cellulose Cuprammonium rayon production Standard solvent for DPv measurement
>64% ZnCl2 >50% Ca(SCN)2 Cl3CHO/DMF
Dissolves cellulose by heating at 100jC Dissolves cellulose by heating at 100jC Dissolves cellulose, forming chloral hemiacetals at all cellulose–OH Dissolves cellulose, forming (poly)methylol hemiacetals at cellulose–OH Dissolves cellulose, forming nitrite ester
(CH2O)x/DMSO N2O4/DMF, N2O4/DMSO
Transparent solution Relatively stable Dissolves cellulose, forming Viscose rayon production system
at LiCl/DMAc, LiCl/DMI SO2/amine/DMSO CH3NH2/DMSO CF3COOH (trifluoroacetic acid: TFA)
all cellulose–OH Stable; needs pretreatments of cellulose Unstable; gives stable amorphous regenerated cellulose Dissolves cellulose, forming complex Dissolves cellulose, forming TFA ester
at (Bu)4N+F ?3H2O/DMSO ca. 80% N-methylmorpholine-N-oxide/H2O Others
NH4SCN/NH3/water N2H4
C6–OH; volatile solvent Dissolves cellulose with DP<650 Uses for lyocell production Dissolves cellulose by heating at 90jC Forms mesophase states Explosive
DMF: N,N-dimethylformamide, DMAc: N,N-dimethylacetamide, DMI: N,N-dimethylimidazolidinone, DMSO: dimethylsulfoxide, Bu: butyl–.
a long time to make viscose rayon and sponge. However, the rayon production, where H2S is emitted more or less during the recovery system of spent liquor, is shrinking because of environmental issues. On the other hand, cellulose is soluble in aqueous NaOH alone under limited conditions. Microcrystalline cellulose with DP 200–300 is soluble in 6–9% NaOH by freezing and defrosting procedures [106]. Pretreatments of cellulose such as steam explosion are necessary for complete dissolution in the aqueous NaOH for normal bleached wood pulp and cotton linters with DP of more than 500 [107]. Many nonaqueous cellulose solvent systems have been developed in the last three decades. Solvent systems consist of reagent(s) reactive to cellulose hydroxyl groups and a polar aprotic solvent such as dimethylsulfoxide (DMSO) or N,N-dimethylacetamide (DMAc). Trifluoroacetic acid is the only volatile solvent to dissolve cellulose [108].
Cellulose hydroxyls form unstable derivatives or complexes with the solvent components in the solution states (Fig. 16). These nonaqueous cellulose solvents were used to prepare cellulose derivatives under homogeneous conditions mainly to control degree of substitutions (DS) and distribution of substituents. The LiCl/DMAc system dissolves cellulose by one of the following two procedures: (1) solvent exchange of cellulose soaked in water to DMAc through ethanol, followed by stirring in 8% LiCl/DMAc at room temperature, (2) heating of cellulose/DMAc suspension at ca. 165jC for 30 min, and LiCl is added to the cellulose suspension at about 100jC in the course of cooling to adjust to 8% LiCl/DMAc [109]. Because cellulose solutions in LiCl/DMAc are fairly stable and powderlike LiCl is easy to handle, these solvent systems were extensively studied as reaction media for homogeneous derivatizations of cellulose. Furthermore, the LiCl/DMAc
148
Atalla and Isogai
added to the solution before spinning in order to avoid strong coloration and oxidative degradation. It is possible to insert an air-gap stage in between spinning nozzles and the water bath for regeneration—hence this system is called ‘‘dry–wet spinning process.’’ Drawing can be achieved in the air-gap stage, resulting in a higher degree of crystallinity as well as a higher degree of orientation of crystals in the regenerated cellulose fiber thereby prepared (Table 2) [111].
III. DERIVATIZATION Because cellulose has three different hydroxyl groups at C2, C3, and C6 in the anhydroglucose unit (Fig. 1), various chemical reactions can possibly apply. Factors influencing the characteristics of cellulose derivatives are as follows: (1) chemical structures of substituents introduced, (2) degree of substitution (DS: the amount of substituents per anhydroglucose unit), (3) distribution of substituents, (4) degree of polymerization and its distribution, (5) purities including the presence of chromophores, and others.
A. Esterification
Figure 16 Dissolving states of cellulose in nonaqueous cellulose solvents.
solvent system has been used as an eluent in size-exclusion chromatographic analyses using a multiangle laser-light scattering (SEC-MALLS) detector for molecular mass and molecular mass distribution of cellulose samples [110]. N-Methylmorpholine-N-oxide (NMMO), containing ca. 20% water, can dissolve cellulose by melting of NMMO at about 90jC, and has recently been used to make regenerated cellulose fiber (lyocell) at industrial level. NMMO is a kind of oxidant, and thus some antioxidant must be
Typical cellulose esters examined so far are depicted in Fig. 17. Cellulose triacetate (DS>2.9) is prepared by heating cellulose suspended in a mixture of acetic anhydride/ acetic acid/H2SO4 around 60jC. Cellulose triacetate is soluble in chlorinated hydrocarbons such as dichloromethane. Cast films of cellulose triacetate have optically characteristic properties of no polarization of penetrated light, and thus have been used as film bases for photograph and supporting films for liquid crystal display. Cellulose diacetate (DS 2.3–2.5) is consecutively prepared from the cellulose triacetate solution by diluting with water and heating. Cellulose diacetate films have been used for ultrafiltration to purify tap water partly in place of chlorination. When pulps having lower a-cellulose content are used, some acetone-insoluble gel fractions originating from hemicellulose are formed from both softwood and hardwood bleached kraft pulps [112]. Thus, bleached sulfite pulp or at least bleached prehydrolyzed kraft pulp prepared from softwood is acceptable as the pulp resources at this point. Therefore, the possibility of using normal
Table 2 Crystallinity Index and Degree of Orientation of Crystals of Regenerated Cellulose Fibers Calculated from their X-ray Diffraction Patterns Cellulose solvent NaOH/CS2/water (viscose rayon) Aqueous Cu(NH3)4(OH)2 (cuprammonium rayon) 6–9% aqueous NaOH 80% NMMO/water (lyocell)
Crystal structure
Crystallinity index (%)
Degree of orientation of crystals (%)
Cellulose II
24
85
Cellulose II
41
90
Cellulose II Cellulose II
46 46
75 91
Developments in Characterization of Cellulose
149
zation media at industrial level. The multicomponent solvent systems, the high boiling point of the solvent such as DMAc and DMSO, the necessity of pretreatments including complete drying of cellulose, and the solventexchanging processes for dissolution are the challenges that would render practical applications of the nonaqueous solvent systems to derivatizations a difficult prospect.
B. Etherification
Figure 17
Typical cellulose esters.
bleached kraft pulp produced from eucalyptus without any spinning problems is one of the significant themes for cellulose diacetate production. Furthermore, one-step production of cellulose diacetate without going through the cellulose triacetate stage is also required. Various cellulose esters such as acetate, tosylate ( ptoluenesulfonate), sinnamoylate, and fluorine-containing substituents were prepared with pyridine as a base under homogeneous and nonaqueous conditions using, for example, 8% LiCl/DMAc. Although interesting results were obtained at the laboratory level, none of these nonaqueous cellulose solvent systems has been applied to the derivati-
Fig. 18 illustrates representative cellulose ethers. In most cases in industries, cellulose ethers are produced via alkalicellulose (cellulose swollen with, e.g., 18% aqueous NaOH) by reacting with etherifying reagents around 60jC in the presence of i-propanol or i-butanol, where etherifications proceed heterogeneously to the swollen alkalicellulose without dissolution. Carboxymethylcellulose sodium salt (CMC), methylcellulose (MC), hydroxyethylcellulose (HEC), and hydroxypropylcellulose (HPC) are typical water-soluble cellulose ethers manufactured at the industrial level, and primarily used as thickeners in various fields. Commercial CMC has DS values in the range of 0.6–1.2. HEC and HPC are produced from alkalicellulose by reacting with ethylene oxide and propylene oxide, respectively. In the case of these cellulose ethers, additional substitution also occurs in hydroxyl groups of the introduced substituents, such as grafting, with increasing the amount of substituents, and thus molecular substitution (MS) in place of DS is used for these cellulose ethers. Water-soluble cellulose ethers in solution states have been characterized by SECMALLS, and the presence of coagulation among cellulose ether molecules in water under particular conditions has been reported [113]. When a small amount of long alkyl chains (C12–C24) are introduced into HEC, viscosity of the aqueous solution extremely increases by the formation of hydrophobic interactions among HEC molecules in water [114]. Nonaqueous media offer an advantageous method to prepare cellulose ethers with high DS, which generally cannot be achieved by the conventional aqueous alkalicellulose system. About 30 kinds of cellulose ethers with DS 3 were prepared by one-step reactions with powdered NaOH and etherifying reagents using the cellulose solution in SO2/ diethylamine/DMSO [115]. The triphenylmethyl (trytyl) group can be selectively introduced at C6 primary hydroxyl of cellulose by homogeneous reaction with pyridine in 8% LiCl/DMAc. This tritylcellulose was used as an intermediate for further conversion to some regioselective cellulose ethers and esters such as 2,3-di-O-methylcellulose and 6-Omethylcellulose (Fig. 19) [116].
IV. OXIDATION There are several methods to modify the chemical structure of cellulose by oxidation. Periodate oxidation of cellulose suspended in water and N2O4 oxidation of cellulose suspended in chloroform are well-known conventional meth-
150
Atalla and Isogai
Figure 18
Typical cellulose ethers.
ods to convert cellulose to dialdehyde cellulose and C6carboxy cellulose, respectively. Generally, however, some side reactions including depolymerization are inevitable during the oxidation process, which makes it difficult to achieve regioselective oxidation completely. 2,2,6,6-Tetramethylpiperidine-1-oxy radical (TEMPO) is a water-soluble and commercially available radical reagent. When sodium hypochlorite is used as a co-oxidant in the presence of catalytic amounts of NaBr and TEMPO in water, C6 primary hydroxyl groups of polysaccharides dissolved in water at pH 10–11 can be selectively converted to carboxyl groups [117]. When this TEMPO-mediated
oxidation is applied to native celluloses, only small amounts of carboxyl groups are introduced into the fibrous celluloses. When regenerated or mercerized, cellulose suspended in water is used as the starting material; on the other hand, water-soluble products are obtained quantitatively at room temperature within 1 h (mostly within 20 min). NMR analyses revealed that these water-soluble oxidized products have homogeneous chemical structures, h-1,4-linked polyglucuronic acid (Fig. 20) [118]. Thus, selective oxidation at C6 primary hydroxyl groups of cellulose can be achieved by TEMPO-mediated oxidation in aqueous media when regenerated or mercerized cellulose
Developments in Characterization of Cellulose
151
Figure 19 Preparation scheme of regioselectively substituted methylcelluloses via tritylcellulose.
is used (Fig. 21). However, some depolymerization of main chains are inevitable. This new water-soluble polyglucuronic acid is degradable to glucuronic acid and hexenuronic acid residues by commercial crude cellulase [119].
specific circumstances, during use. The quality of cellulosic materials is reduced through degradation by means of these outside stimuli. On the other hand, if these degradations can be well controlled, useful cellulose-related compounds can be obtained.
V. DEGRADATION
A. Acid Hydrolysis
Cellulosic materials undergo numerous and sometimes harsh stimuli during manufacturing processes and, under
Acid hydrolysis of cellulosic biomass can be used to produce glucose, which is then converted to ethanol by
152
Atalla and Isogai
fermentation. Susceptibility of cellulosic materials to acid hydrolysis is remarkably different between their ordered and disordered regions. When native cellulosic materials such as cotton linters and bleached chemical wood pulps are heated in a dilute acid, hydrolysis of disordered regions in cellulose microfibrils precedes that of ordered regions to form the so-called ‘‘microcrystalline cellulose’’ with DP 200–300. A part of glucose once formed from cellulose by acid hydrolysis is further degraded to hydroxymethylfurfural, levulinic acid, formic acid, and others during acid hydrolysis (Fig. 22).
B. Enzymatic Degradation
Figure 20 13C NMR spectra of cellulose oligomer (DP 7) in DMSO and cellouronic acid Na salt (h-1,4-linked polyglucuronic acid) in D2O. Cellouronic acid Na salt was prepared from viscose rayon by the TEMPO-mediated oxidation.
Figure 21
Cellulase hydrolyzes cellulose under mild conditions compared with inorganic or organic acid. Generally, cellulases such as cellobiohydrolase II (CBH II) consist of core and cellulose-binding domains and a linker, which binds the two domains. The core domain contains an active center to hydrolyze cellulose in catalytic manner and the subsites, which interact with cellulose chain close to the active center. The cellulose-binding domains consist of amino
TEMPO-mediated oxidation of C6 primary hydroxyl group of cellulose to carboxyl group.
Developments in Characterization of Cellulose
Figure 22
Figure 23
153
Some degradation products of cellulose.
Classification of cellulase into processive and nonprocessive types.
154
Atalla and Isogai
Figure 24
Enzymatic synthesis of cellulose from h-cellobiosyl fluoride in acetonitrile/aqueous buffer mixture.
acids having aromatic rings such as tyrosin or triptophan, and these aromatic rings of the cellulose-binding domains attach to hydrophobic plains of cellulose chains through van der Waals force. The active center of the core domains of cellulase can then attack the cellulose chain. The subsites of the core domains can give some mechanical stress to the cellulose chain, and one of glucose residues of the cellulose chain compulsorily have the unstable boat form. Thus, remarkable reduction of activation energy to hydrolyze cellulose can be achieved [120]. Various types of cellulase have been reported so far, and they have been, for a long time, classified into two types—exo- and endocellulases—depending on whether or not the cellulase can recognize the reducing ends of cellulose chains. Cellobiohydrolase (CBH) and endoglucanase (EG) are then further categorized into two types. However, recent studies revealed that there are no exo-type cellulases, and that all cellulases are included in the endo-type. On the other hand, the following classification are now well accepted: the processive and nonprocessive cellulases on
Figure 25
the basis of hydrolysis patterns of cellulose chains (Fig. 23) [121].
C. Thermal Degradation When cellulose is analyzed by thermogravimetry under nitrogen atmosphere, thermal decomposition starts at 200–270jC, depending on the purity of cellulose samples. The temperature of ignition in the air is in the range of 390– 420jC, and the maximum flame temperature reaches 800jC or more. When cellulose is heated at temperatures exceeding 100jC under reduced pressure, levoglucosan (Fig. 22) is obtained in the maximum yield of 70%. When thermal carbonization is applied to cellulosic materials under inactive gas atmosphere, the yields of carbon are lower than the theoretical value (44%) because a part of cellulose is converted to levoglucosan. Yields of carbon can be increased by adding hydrochloric acid, which enhances dewatering rather than the formation of levoglucosan
Chemical syntheses of cellulose.
Developments in Characterization of Cellulose
[122]. When cellulose microcrystals, which are obtained from crystalline native celluloses by acid hydrolysis, are carbonized under suitable conditions, carbon nano-lods are obtained [123]. Microwave treatment is one of the heating methods used, in which more homogeneous heating can be achieved, compared with the thermal conduction-type heating. Saccharification of lignocellulosics has been studied from this aspect, and the maximum yield of glucose was reported to be 81% based on theoretical value [124]. Two of the thermal treatments, explosion and laser irradiation treatments, were employed to obtain glucose and levoglucosan. Supercritical water treatment is also one of the heating methods in the presence of acid. Dissociation of water can increase under supercritical conditions, and thus water behaves like an acid catalyst to cellulose. Noncatalytic hydrolysis of cellulose can, therefore, be achieved by supercritical water treatments. The maximum yield of glucose was reported to be in the range of 32–48% [125].
155
reactions and conformational restrictions for polymerization of carbohydrate monomers [128].
REFERENCES 1. 2. 3. 4. 5. 6. 7. 8. 9. 10.
VI. CHEMICAL AND ENZYMATIC SYNTHESES OF CELLULOSE Although cellulose is one of the naturally occurring polysaccharides, artificial synthesis of cellulose from monomers or dimers has been of scientific interest for a long time. Syntheses of cellulose have recently been succeeded by the following two different principles. Cellulase hydrolyzes the h-1,4-glucoside bonds of cellulose, and this enzymatic hydrolysis is essentially reversible. Kobayashi et al. [126] successfully carried out cellulose synthesis by using the reversible reaction of cellulase, where a particular substrate, h-cellobiosyl fluoride, was used in an aqueous buffer containing acetonitrile (Fig. 24). The origin and purity of cellulase and combination of the solvent systems influenced the yields of synthesized cellulose and its crystal structure. Cellulase from Trichoderima viride gave the highest yield, ca. 54%, of water-insoluble, low-molecular weight cellulose (DP 22), whereas h-glucosidase yielded no cellulose. Generally, the enzymatically synthesized cellulose has the crystal structure of cellulose II, which is the same as that of regenerated or mercerized cellulose. On the other hand, cellulose bearing the crystal structure of cellulose I, which is the same as that of native cellulose, was synthesized in vitro by using a highly purified cellulase component [127]. Cellulose oligomers and low-DP cellulose have been prepared by the following three routes and the successive elimination of the protecting groups at hydroxyl groups: (1) linear synthetic reaction using the imidate method from allyl 2,3,6-tri-O-benzyl-4-O-p-methoxybenzyl-h-D-glucopyranoside, (2) confluent-type reaction between cellotetraose and cellooctaose derivatives using the imidate method, and (3) cationic ring-opening polymerization of glucose 1,2,4-orthoester (Fig. 25). These studies revealed the roles of specific protecting groups at particular hydroxyl positions of the starting materials in regioselective
11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29.
30. 31.
Atalla, R.H. In Comprehensive Natural Products Chemistry, Carbohydrates; Pinto, B.M., Ed.; Elsevier: London, 1999; Vol. 3, 529–598. Gardner, K.H.; Blackwell, J. Biopolymers 1974, 13, 1975. Hebert, J.J.; Muller, L.L. J. Appl. Polym. Sci. 1974, 18, 3373. Meyer, K.H.; Misch, L. Helv. Chim. Acta 1937, 20, 232. Hermans, P.H. Physics and Chemistry of Cellulose Fibers; Elsevier: New York, 1949. French, A. In The Structures of Celluloses, ACS symposium Series 340; Atalla, R.H., Ed.; American Chemical Society: Washington, DC, 1987; 15 pp. Pauling, L. The Nature of the Chemical Bond, 3rd Ed.; Cornell University Press: Ithaca, NY, 1960; 65 pp. Woodward, L.A. Introduction to the Theory of Molecular Vibrations and Vibrational Spectroscopy; Oxford University Press: Oxford, 1972; 344 pp. Atalla, R.H. Appl. Polym. Symp. 1976, 28, 659. Pitzner, L.J. The Vibrational Spectra of the 1,5-anhydropentitols, Doctoral dissertation; The Institute of Paper Chemistry: Appleton, WI, 1973. Pitzner, L.J.; Atalla, R.H. Spectrochim. Acta 1975, 31A, 911. Watson, G.M. The Vibrational Spectra of the Pentitols and Erythritol, Doctoral Dissertation; The Institute of Paper Chemistry: Appleton, WI, 1974. Edwards, S.L. The Vibrational Spectra of the Pentose Sugars, Doctoral Dissertation; The Institute of Paper Chemistry: Appleton, WI, 1976. Williams, R.M. The Vibrational Spectra of the Inositols, Doctoral Dissertation; The Institute of Paper Chemistry: Appleton, WI, 1977. Williams, R.M.; Atalla, R.H. J. Phys. Chem. 1984, 88, 508. Wells, H.A. The Vibrational Spectra of Glucose, Galactose and Mannose, Doctoral Dissertation; The Institute of Paper chemistry: Appleton, WI, 1977. Wells, H.A.; Atalla, R.H. J. Mol. Struct. 1990, 224, 385. Carlson, K.P. The Vibrational Spectra of the Cellodextrins, Doctoral Dissertation; The Institute of Paper Chemistry: Appleton, WI, 1978. Wiley, J.H.; Atalla, R.H. Carbohydr. Res. 1987, 160, 113. Rees, D.A.; Skerret, R.J. Carbohydr. Res. 1968, 7, 334. Petipas, T.; Oberlin, M.; Mering, J. J. Polym. Sci. C 1963, 2, 423. Norman, M. Text. Res. J. 1963, 33, 711. Sarko, A.; Muggli, R. Macromoles 1974, 7, 486. Chu, S.S.C.; Jeffrey, G.A. Acta. Crystallogr. 1968, B24, 830. Ham, J.T.; Williams, D.G. Acta. Crystallogr. 1970, B29, 1373. Wilson, E.B., Jr.; Decius, J.C.; Cross, P.c. Molecular Vibrations; McGraw-Hill: New York, 1955; 188 pp. Nelson, M.L.; O’Connor, R.T. J. Appl. Polym. Sci. 1964, 8, 1311. Melberg, S.; Rasmussen, K. Carbohydr. Res. 1979, 71, 25. Henrissat, B.; Perez, S.; Tvaroska, I.; Winters, w.T. In The Structures of Celluloses, ACS symposium Series 340; Atalla, R.H., Ed.; American Chemical Society: Washington, DC, 1987; 38 pp. Atalla, R.H. Adv. Chem. Ser. 1979, 181, 55. Atalla, R.H.; Gast, J.C.; Sindorf, D.W.; Bartuska, V.J.; Maciel, G.E. J. Am. Chem. Soc. 1980, 102, 3249.
156 32. Atalla, R.H. Proceedings of the International Symposium on Wood and Pulping Chemistry, SPCI Rept. No 38, Stockholm 1981, 1, 57. 33. Atalla, R.H. In Structure, Function and Biosynthesis of Plant Cell Walls; Dugger, W.M., Bartinicki-Garcia, S., Eds.; American Society of Plant Physiologists: Rockville, MD, 1984. 381 pp. 34. Atalla, R.H. J. Appl. Pol. Sci., Appl. Pol. Symp. 1983, 37, 295. 35. Earl, W.L.; VanderHart, D.L. J. Am. Chem. Soc. 1980, 102, 3251. 36. Earl, W.L.; VanderHart, D.L. Macromoles 1981, 14, 570. 37. D.L. VanderHart, Deductions about the morphology of wet and wet beaten cellulose from solid state 13C NMR, NBSIR 82-2534. 38. Fyfe, C.A.; Dudley, R.L.; Stephenson, P.J.; Deslandes, Y.; Hamer, G.K.; Marchessault, R.H. J. Am. Chem. Soc. 1983, 105, 2469. 39. Horii, F.; Hirai, A.; Kitamaru, R. Polym. Bull. 1982, 8, 163. 40. Maciel, G.E.; Kolodziejski, W.L.; Bertran, M.S.; Dale, B.R. Macromoles 1982, 15, 686. 41. Gast, J.C.; Atalla, R.H.; McKelvey, R.D. Carbohydr. Res. 1980, 84, 137. 42. VanderHart, D.L.; Atalla, R.H. Macromoles 1984, 17, 1465. 43. Atalla, R.H.; VanderHart, D.L. Science 1984, 223, 283. 44. Howsmon, J.A.; Sisson, W.A. In Cellulose and Cellulose Derivatives, Pt. I; Ott, E., Spurlin, H.M., Graffline, M.W., Eds.; Interscience: New York, 1954; 237 pp. 45. Blackwell, J.; Marchessault, H. In Cellulose and Cellulose Derivatives, Pt. IV; Bikales, N.M., Segal, L., Eds.; WileyInterscience: New York, 1971; 1 pp. 46. VanderHart, D.L.; Atalla, R.H. In The Structures of Celluloses, ACS Symposium Series 340; Atalla, R.H., Ed.; American Chemical Society: Washington, DC, 1987; 88 pp. 47. Atalla, R.H.; Whtimore, R.E.; VanderHart, D.L. Biopolymers 1985, 24, 421. 48. Horii, F.; Yamamoto, H.; Kitamaru, R.; Tanahashi, M.; Higuchi, T. Macromoles 1987, 20, 2946. 49. Wiley, J.H.; Atalla, R.H. In The Structures of Celluloses, ACS Symposium Series 340; Atalla, R.H., Ed.; American Chemical Society: Washington, DC, 1987; 151 pp. 50. Sugiyama, J.; Presson, J.; Chanzy, H. Macromoles 1990, 24, 4168. 51. Yamamoto, H.; Horii, F.; Odani, H. Macromolecules 1989, 22, 4130. 52. Sugiyama, J.; Okano, T.; Yamamoto, H.; Horii, F. Macromoles 1990, 23, 3196. 53. Atalla, R.H.; Hackney, J.; Agarwal, U.P.; Isogai, A. Int. J. Biol. Macromol. in press. 54. Bower, D.I.; Maddams, W.F. The Vibrational Spectroscopy of Polymers; Cambridge University Press: Cambridge, UK, 1989. 55. Horri, F.; Hirai, A.; Kitamaru, R. The Structures of Celluloses, ACS Symposium Series 340; Atalla, R.H., Ed.; American Chemical Society: Washington, DC, 1987; 119 pp. 56. VanderHart, D.L.; Campbell, G.C. J. Magn. Reson. in press. 57. Yamamoto, H.; Horii, F. Macromoles 1993, 26, 1313. 58. Yamamoto, H.; Horii, F.; Odani, H. Macromoles 1989, 22, 4130. 59. Yamamoto, H.; Horii, F. Macromoles 1993, 26, 1313. 60. Belton, P.S.; Tanner, S.F.; Cartier, N.; Chanzy, H. Macromoles 1989, 22, 1615. 61. Yamamoto, H.; Horii, F. Cellulose 1994, 1, 57. 62. Newman, R.H.; Hemmingson, J.A. Holzforschung 1990, 44, 351.
Atalla and Isogai 63. Newman, R.H.; Hemmingson, J.A. Cellulose 1995, 2, 95. 64. Newman, R.H. J. Wood Chem. Technol. 1994, 14, 451. 65. Newman, R.H.; Ha, M.A.; Melton, L.D. J. Agric. Food Chem. 1994, 42, 1402. 66. Newman, R.H.; Davies, L.M.; Harris, P.J. Plant Physiol. 1996, 111, 474. 67. Newman, R.H. Cellulose 1997, 4, 269. 68. Lenholm, H.; Larsson, T.; Iversen, T. Carbohydr. Res. 1994, 261, 119. 69. Lennholm, H.; Larsson, T.; Iversen, T. Carbohydr. Res. 1994, 261, 119. 70. Larsson, T.; Westermark, U.; Iversen, T. Carbohydr. Res. 1995, 278, 339. 71. Larsson, T.; Wickholm, K.; Iversen, T. Carbohydr. Res. 1997, 302, 19. 72. Hock, C.W. In Cellulose and Cellulose Derivatives, Pt. I; Ott, E., Spurlin, H.M., Grafflin, M.W., Eds.; Interscience: New York, 1954; 347 pp. 73. Morehead, F.F. In Cellulose and Cellulose Derivatives, Pt. IV; Bikales, N.M., Segal, L., Eds.; Wiley-Interscience: New York, 1971; 213 pp. 74. Preston, R.D. The Physical Biology of Plant Cell Walls; Chapman & Hall: London, 1974. 75. Hieta, K.; Kuga, S.; Usuda, M. Biopolymers 1984, 23, 1807. 76. Chanzy, H.; Henrissat, B. FEBS Lett. 1985, 184, 285. 77. Maurer, A.; Fengel, D. Holz als Roh- und Werkstoff 1992, 50, 493. 78. Sugiyama, J.; Harada, H.; Fujiyoshi, Y.; Uyeda, N. Mokuzai Gakkaishi 1984, 30, 98. 79. Sugiyama, J.; Harada, H.; Fujiyoshi, Y.; Uyeda, N. Mokuzai Gakkaishi 1985, 31, 61. 80. Sugiyama, J.; Harada, H.; Fujiyoshi, Y.; Uyeda, N. Planta 1985, 166, 161. 81. Frey-Wyssling, A. The Plant Cell Wall; Gebruder Borntrager: Berlin, 1976. 82. Sugiyama, J.; Okano, T.; Yamamoto, H.; Horii, F. Macromoles 1990, 23, 3196. 83. Honjo, G.; Watanabe, M. Nature 1958, 181, 326. 84. Sugiyama, J.; Vuong, R.; Chanzy, H. Macromoles 1991, 24, 4168. 85. Roche, E.; Chanzy, H. J. Biol. Macromol. 1981, 3, 201. 86. Ellefsen, 0.; Tonessen, B.A. In Cellulose and Cellulose Derivatives, Pt. IV; Bikales, N.M., Segal, L., Eds.; WileyInterscience: New York, 1971; 151 pp. 87. Chanzy, H.; Henrissat, B.; Vincendon, M.; Tanner, S.; Belton, P.S. Carbohydr. Res. 1987, 160, 1. 88. Atalla, R.H.; Dimick, B.E.; Nagel, S.C. In Cellulose Chemistry and Technology; Arthur, J.C. Jr., Ed.; ACS Symp. Series No. 40, American Chemical Society: Washington, DC, 1977; 30 pp. 89. Atalla, R.H.; Ellis, J.D.; Schroeder, L.R. J. Wood Chem. Technol. 1984, 4, 465. 90. Chanzy, H.; Imada, K.; Mollard, A.; Vuong, R.; Barnoud, F. Protoplazma 1979, 100, 303. 91. Bertoniere, N.R.; Zeronian, S.H. In The Structures of Celluloses, ACS Symposium Series 340; Atalla, R.H., Ed.; American Chemical Society: Washington, DC, 1987; 255 pp. 92. Rowland, S.P.; Roberts, E.J. J. Pol. Sci. A-1 1972, 10, 2447. 93. Nickerson, R.F. Text. Res. J. 1951, 21, 195. 94. Rowland, S.P.; Roberts, E.J.; Wade, C.P. Text. Res. J. 1969, 39, 530. 95. Rowland, S.P. In Modified Cellulosics; Rowell, R.M., Young, R.A., Eds.; Academic Press: New York, 1978; 147 pp. 96. Rowland, S.P.; Roberts, E.J.; Bose, J.L. J. Pol. Sci. A-1 1971, 9, 1431. 97. Rowland, S.P.; Roberts, E.J.; Bose, J.L.; Wade, C.P. J. Pol. Sci. A-1 1971, 9, 1623.
Developments in Characterization of Cellulose 98. Mann, J.; Marinan, H.J. J. Polym. Sci. 1958, 32, 357. 99. Zeronian, S.H.; Coole, M.L.; Alger, K.W.; Chandler, J.M. J. Appl. Pol. Sci., Appl. Pol. Symp. 1983, 37, 1053. 100. Stone, J.E.; Scallan, A.M. Pulp Pap. Mag. Can. 1968, 69, 69. 101. Stone, J.E.; Treiber, E.; Abrahamson, E. TAPPI 1969, 28, 139. 102. Bell, R.P. The Proton in Chemistry; Cornell University Press: Ithaca, NY, 1973. 103. Johnson, D.C.; Nicholson, M.D.; Haigh, F.C. Appl. Polym. Symp. 1976, 28, 931. 104. Johnson, D.C.; Nicholoson, M.D. Cellul. Chem. Technol. 1977, 11, 349. 105. Isogai, A. Chemical modification of cellulose. In Wood and Cellulosic Chemistry; Hon, D.N.-S., Shiraishi, N., Eds.; Mercer Dekker: New York, 2000, 599–625. 106. Isogai, A.; Atalla, R.H. Dissolution of cellulose in aqueous NaOH solutions. Cellulose 1998, 5, 309–319. 107. Kamide, K.; Okajima, K.; Kowsaka, K. Dissolution of natural cellulose into aqueous alkali solutions: Role of supermolecular structure of cellulose. Polym. J. 1992, 24, 71–86. 108. Isogai, A.; Atalla, R.H. Preparation of cellulose–chitosan polymer blends. Carbohydr. Polym. 1992, 19, 25–28. 109. Turbak, A.F., El-Kafrawy, A., Snyder, F.W., Jr., Auerbach, A.B., Solvent system for cellulose, U.S. Pat., 4302252 (1981). 110. Schult, T.; Hjerde, T.; Optun, O.I.; Kleppe, P.J.; Moe, S. Characterization of cellulose by SEC-MALLS. Cellulose 2002, 9, 149–158. 111. Okajima, K.; Yamane, C. Cellul. Commun. 1997, 4, 7–12. 112. Saka, S.; Takahashi, K.; Matsumura, H. Effects of solvent addition to acetylation medium on cellulose triacetate prepared from low-grade hardwood dissolving pulp. J. Appl. Polym. Sci. 1998, 69, 1445–1449. 113. Jumel, K.; Harding, S.E.; Mitchell, J.R.; To, K.-M.; Hayter, I.; O’Mullane, J.E.; Ward-Smith, S. Carbohydr. Polym. 1996, 29, 105–109. 114. Tanaka, R.; Meadows, J.; Phillips, G.O.; Williams, P.A. Viscometric and spectroscopic studies on the solution behavior of hydrophobically modified cellulosic polymers. Carbohydr. Polym. 1990, 12, 443–459. 115. Isogai, A.; Ishizu, A.; Nakano, J. Preparation of tri-Oalkylcelluloses by the use of a non-aqueous cellulose solvent and their physical characteristics. J. Appl. Polym. Sci. 1986, 31, 341–352.
157 116.
117.
118. 119.
120. 121. 122. 123. 124.
125. 126.
127. 128.
Kondo, T.; Gray, D.G. The preparation of O-methylcellulosese and O-ethylcelluloses having controlled distribution of substituents. Carbohydr. Res. 1991, 220, 173– 183. de Nooy, A.E.J.; Besemer, A.C.; Bekkum, H. Highly selective nitroxyl radical-mediated oxidation of primary alcohol groups in water-soluble glucans. Carbohydr. Res. 1995, 269, 89–98. Isogai, A.; Kato, Y. Preparation of polyuronic acid from cellulose by TEMPO-mediated oxidation. Cellulose 1998, 5, 153–164. Kato, Y.; Habu, N.; Yamaguchi, J.; Kobayashi, Y.N.; Shibata, I.; Isogai, A.; Samejima, M. Biodegradation of h1,4-linked polyglucuronic acid (cellouronic acid). Cellulose 2002, 9, 75–81. Henrissat, B. Cellulases and their interaction with cellulose. Cellulose 1994, 1, 169–196. Davies, G.; Henrissat, B. Structures and mechanisms of glycosyl hydrolases. Structure 1995, 3, 853–859. Kim, D.Y.; Nishiyama, Y.; Wada, M.; Kuga, S. High-yield carbonization of cellulose by sulfuric acid impregnation. Cellulose 2001, 8, 29–33. Kuga, S.; Kim, D.Y.; Nishiyama, Y.; Brown, R.M. Nanofibrillar carbon from native cellulose. Mol. Cryst. Liq. Cryst. 2002, 387, 237–243. Azuma, J.; Asai, T.; Isaka, M.; Koshijima, T. Microwave irradiation of lingocellulosic materials. 5. Effects of microwave irradiation on enzymatic susceptibility of crystalline cellulose. J. Ferment. Technol. 1985, 63, 529–536. Saka, S.; Ueno, T. Chemical conversion of various celluloses to glucose and its derivatives in supercritical water. Cellulose 1999, 6, 177–191. Kobayashi, S.; Kashiwa, K.; Kawasaki, T.; Shoda, S. Novel method for polysaccharide synthesis using an enzyme—The first in vitro synthesis of cellulose via a nonbiosynthetic path utilizing cellulase as catalyst. J. Am. Chem. Soc. 1991, 113, 3079–3084. Lee, J.H.; Brown, R.M.; Kuga, S.; Shoda, S.; Kobayashi, S. Assembly of synthetic cellulose I. Proc. Natl. Acad. Sci. U. S. A. 1994, 91, 9195. Nakatsubo, F.; Kamitakahara, H.; Hori, M. Cationic ringopening polymerization of 3,6-di-O-benzyl-alpha-D-glucose 1,2,4-orthopivalate and the first chemical synthesis of cellulose. J. Am. Chem. Soc. 1996, 118, 1677–1681.
6 Two-Dimensional Fourier Transform Infrared Spectroscopy Applied to Cellulose and Paper Lennart Salme´n and Margaretha A˚kerholm STFI (Swedish Pulp and Paper Research Institute), Stockholm, Sweden
Barbara Hinterstoisser BOKU-University of Natural Resources and Applied Life Sciences, Vienna, Austria
I. INFRARED SPECTROSCOPY FOR WOOD AND CELLULOSE RESEARCH An infrared spectrum contains the complete information about the molecular assembly of a material or a substance. This fact made infrared (IR) spectroscopy a widely used analytical tool especially, but not exclusively, for identifying and characterizing the molecular structure of organic compounds. IR spectroscopy has therefore a long tradition in organic chemistry and was, for a substantial length of time, among the main spectroscopic tools for elucidating the chemical structure of purified substances. IR spectroscopy has also for a long time been a useful analytical method for wood and cellulose chemistry. Even in the 1940s, it was used to investigate the native structure of lignin [1,2]. Over the years, it was developed and used for determining the composition of lignin, cellulose, and hemicelluloses in wood and pulps, for studying derivatives and model compounds of these polymers, as well as for studying changes caused by heat or chemical treatment as used in various processes (e.g., Refs. [3–20]). In Fig. 1, an overview of the band assignments of an IR spectrum of cellulose is shown as a guide to accompany the text in this chapter. Although the IR spectra of cellulose contain several overlapping bands making them difficult to interpret, IR spectroscopy has been used for more than 50 years as an ‘‘accompanying’’ technique for wood and cellulose chemistry to estimate the crystallinity of cellulose; some important work was carried out by Mann and Marrinan [21,22]. These IR studies were based on the reaction of cellulose with heavy water. Tsuboi [5] early on assigned a number of bands for cellulose and worked out differences between
cellulose I, cellulose II, and amorphous cellulose using polarized IR radiation. A further important investigation was carried out on mercerized cellulose and wood polysaccharides by Liang and Marchessault [6,7,23–25], who estimated the crystallinity of cellulose and assigned specific cellulose-, lignin-, and hemicellulose-deriving bands by IR spectrometry. When Liang and Marchessault [6] in 1959 wrote about native celluloses, a large part of their publication questioned the possibilities of hydrogen bonding. They found a strong parallel OH stretching band vibrating in-phase with all C3 hydroxyl groups (3350 cm1). They attributed it to an intramolecular hydrogen bond between the hydroxyl group on the C3 atom of one glucose residue and the ring oxygen of the next residue, a bond which is subsequently referred to as O3H. . .O5V in the text. Referring to their IR data, they also discussed other possibilities of hydrogen bonding, for example, between the hydroxyl group of the C6 and the bridge oxygen of the glycosidic linkage. Furthermore, there was a proposal that the C6 hydroxyl group might be bonded either to the oxygen of the C2 of the next glucose ring, bifurcated between the bridge oxygen and the oxygen of the C2 of the next ring, or that the hydroxyl group at the C2 might be bonded to the C6 oxygen. It was suggested that intermolecular hydrogen bonds might exist between the C6 hydroxyl group of one chain and the bridge oxygen of the neighboring chain. The weaker bands at 3405 and 3305 cm1 in the IR spectra of bacterial celluloses were ascribed to intermolecular hydrogen bonds. It was proposed that a fourth band found at 3245 cm1 was also derived from intermolecular hydrogen bonds. This band at 3245 cm1 was found only in bacterial and algae celluloses but not for cotton and ramie. 159
160
Salme´n et al.
Figure 1 The static FT-IR spectrum of a spruce dissolving pulp cellulose together with an overview of the band assignments.
In 1963, Smith et al. [26] again used infrared spectroscopy to determine the degree of crystallinity of cellulose using deuterated samples. Nelson and O’Connor [27] compared highly crystalline cellulose samples of different lattice types (I, II, and III) and amorphous cellulose, focusing on the spectral region between 850 and 1500 cm1. They questioned the use of bands at 1420, 893– 897, and 1111 cm1 for estimating crystallinity for mixed lattice types as done by other authors. The stabilizing function of intramolecular hydrogen bonds was discussed as well. Tritium exchange was another attempt to obtain more knowledge of crystallinity and the accessibility of hydrogen bonds using IR spectroscopy as a detection system [28]. Ra˚nby concluded that in dry cellulose, less than 1% of the hydroxyl groups exist as free groups and that in the crystalline regions, all hydroxyl groups are involved in bonding. The possible applications of IR spectroscopy to the qualitative and quantitative testing of pulp and paper were reviewed in 1965 by Jayme and Rohmann [29]. Several papers have dealt with trials to unravel the broad OH region, which hides all the structure-relevant information relating to hydrogen bonding. An overview of band assignments carried out up to 1972 was given by Dechant et al. [30]. Siesler et al. [11] described a technique for the measurement of the plane-polarized IR spectra of deuterated cellulosic fibers by frustrated multiple internal reflectance (FMIR). Their aim was to investigate regenerated cellulose fibers according to the molecular orientation
of the polymer chains. Their investigations were based on the fact that the dichroism of the crystalline OH stretching vibrations is related to the molecular orientation as a result of the extent of stretching of the cellulose fibers. In the following years, several papers were published dealing with determinations of the degree of crystallinity (e.g., Refs. [31–33]). While in the ‘‘old days,’’ samples in a solid or liquid state were measured by dispersive working instruments, the 1980s brought a renaissance of IR spectroscopy through the introduction of the Fourier transform (FT) technique. While the former dispersive instruments contained a monochromator which provided one welldefined wavelength range after the other to which the sample was exposed, FT-IR instruments irradiate the sample with an interference wave produced in an interferometer. The interferogram recorded by the detector is related to the spectrum through its Fourier transform. The fact that the radiation reaching the detector contains all wavelengths at one time gives the so-called multiplex (or Fellgett) advantage. It allows spectra of the same signal-tonoise ratio (SNR) to be measured much faster on an FT-IR spectrometer than on a traditional dispersive instrument. Another outstanding advantage is given by the optical throughput (Jacquinot advantage), which is greater for an interferometer than for a monochromator. The invention of the Fourier transform infrared (FT-IR) technique opened up new possibilities in instrumentation and in the coupling of analytical systems as well as in the application
2D FT-IR Spectroscopy Applied to Cellulose and Paper
of specific software facilities. This includes, for example, the possibility of mathematical processing of the spectra, such as differentiation to give the second derivative [34], and deconvolution of spectra [16,18,35], all of which provide better resolution of the absorption bands. The deconvolution of the range of the OH stretching vibrations gives detailed evidence of crystallinity, crystal modification, and degree of substitution of cellulose and cellulose derivatives [36]. However, neither deconvolution nor differentiation increases the instrumental resolution; they are merely methods for resolving overlapping bands by computation [34,37]. Progress in FT-IR spectroscopy led to investigations not only of molecular structures, but also of pattern recognition in complex systems, as well as qualitative and quantitative assessment of components as pure substances or within complex matrices like wood [13,38,39]. Additionally, several sophisticated techniques, such as, for example, attenuated total reflection (ATR), photoacoustic, and diffuse reflection FT-IR (DRIFT), and instrument couplings between FT-IR and gas chromatography (GC), high-performance liquid chromatography (HPLC), or thermogravimetric analyzers (TGA) provided further possibilities for solving analytical questions [40–43]. This also resulted in new application possibilities for wood and pulping chemistry [41]. A third point to be mentioned is that an extremely high wave number precision is obtained by the FT-IR technique. One of the promising (new) techniques was FT-IR microspectroscopy, which made possible the investigation of very small samples with diameters of about 10– 50 Am [44]. Ludwig and Fengel [45] used FT-IR microscopy to study cellulose nitrate fibers of different degrees of substitution. In the 1990s, focus was drawn to the allomorphic forms of native cellulose, namely, cellulose Ia and cellulose Ih. FT-IR spectroscopy, besides electron diffraction studies, electron microscopy, and CP/MAS 13C-NMR spectroscopy, was one of the techniques used [17,46–49]. The IR bands between 400 and 800 cm1, as well as the region of the OH stretching vibration, turned out to be of interest in investigating the polymorphism of native cellulose. Absorption bands near 3240 and 750 cm1 were assigned to the triclinic cellulose Ia phase. The bands near 3270 and 710 cm1 were assigned to the monoclinic cellulose Ih phase. The crystallinity of cellulose remained of great interest in investigations of higher plants [42, 50], algae [51], and cell wall formation [52], as well as for pulp and paper research [53,54]. Associated with the allomorphic forms, the hydrogen bonding pattern also remained a topic of interest [55]. With the development of a combination of dynamic mechanical analysis (DMA) and IR spectroscopy, new possibilities were seen for assigning and interpreting spectra of biopolymers like cellulose. Starting in the late 1990s, this technique was applied to investigate cellulose, in particular, the hydrogen bonding, the allomorph composition, the stretching behavior, and the interactions within the wood polymer network also including hemicelluloses and lignin [20,56–61].
161
II. TWO-DIMENSIONAL FOURIER TRANSFORM INFRARED SPECTROSCOPY In polymer research, IR spectroscopy has been and is still applied to identify and determine chemical composition, including end groups and chain branching of the polymers. The configuration and conformation, as well as steric and geometric isomerism, is a further area that, to some extent, can be unraveled [40,62]. To obtain such information on polymers is of great importance since the mechanical properties, such as strength, ductility, and glass transition temperature, are a result of the organization and orientation of the polymer chains and of the molecular structure in general. IR spectroscopy, even in the 1970s, was a proven technique which allowed statements about structural changes relating to deformation through external stress [11]. All these measurements had, however, been based on static studies. Time-resolved IR spectroscopy (TRS) was proposed in the 1980s as a new tool for dynamic studies to investigate the deformation behavior of polymers [63]. Burchell and Hsu [63] connected a computer-controlled hydraulic stretching device, providing a predefined periodic oscillatory strain to an FT-IR spectrometer working in rapid scanning mode. An important point was that the applied strain had to be far below the yield point, namely, in the linear region of the stress–strain diagram. In general, the idea was that if the directions of the dipole transition moments with respect to the chain axis were known, stress-induced changes in orientation, conformation, and packing could be measured. Therefore it was necessary to establish and calibrate the changes in the FT-IR spectra (e.g., frequency, intensity, vibrational bandwidth, and dichroism) as a function of the strain amplitude and the strain rate. This led to the possibility of directly assigning the molecular dipole transition moments involved in stressinduced intramolecular changes via the obtained changes in the absorption bands. Furthermore, direction-dependent orientational, conformational, and packing changes could also be observed. FT-IR spectroscopy now provided a tool for not only static, but also dynamic measurements. In the following years, time-resolved IR spectroscopy became more and more recognized as a promising technique for polymer research [64,65]. Lasch et al. [66] studied polymer deformations by slowly stretching oriented polymer films while IR-spectrometrically studying changes in the macromolecular structure. In these experiments, the stretcher, which provided the stress to the polymer sample, was run continuously and not synchronized to the interferometer. Therefore all the data were collected and all interferograms with identical phases had to be co-added. The combination of IR spectroscopy and mechanical (so-called rheo-optical) measurements led to more detailed data and therefore to a better understanding of the mechanisms involved in polymer deformation. Noda et al. [67] constructed a system designed to detect dynamic IR linear dichroism (DIRLD) in polymer samples undergoing small oscillatory strains using a dispersive IR instrument. Small amplitude oscillatory strain was applied to thin films of
Salme´n et al.
162
quency, x, to the sample, the dynamic signal A˜(m,t) from the sample can be written as ˜ tÞ ¼ AðmÞsin½xt ˆ Aðm; þ bðmÞ
Figure 2 Schematic drawing of a dynamic FT-IR experiment.
polyethylene mounted in a stretching device. The polarization of the IR beam was altered at a very high frequency between parallel and perpendicular directions (i.e., with respect to the stretching). Dichroic differences between the absorbances parallel and perpendicular to the stretch direction as small as 5105 with a time resolution of better than 14 Asec were detected. The development of the dynamic IR linear dichroism technique turned out to be fast and sensitive enough to detect molecular level relaxations of strain-induced orientations in polymers, although these orientations occur and relax very rapidly. Polymers such as isotactic polypropylene served as model compounds in the development of the new technique. In 1987, Noda et al. [68] compared Fourier transform and dispersive spectroscopy in the characterization of polymers in polarization–modulation IR techniques. By that time, the dispersive instrument had been given preference. In 1991, Palmer et al. [69] introduced FT-IR spectroscopy to perform such dynamic experiments. A technical improvement—the step scan interferometry— allowed advantage to be taken of FT-IR as well as of the two-dimensional correlation and coupling to dynamic mechanical analysis (DMA). As the step-scanning decouples the spectral multiplexing from the time domain, the time dependence of the sample response to the external perturbation was shown to be regained quite easily [70]. Again, an external sinusoidal small amplitude strain is applied to a sample that is irradiated with polarized IR light (Fig. 2). The time-dependent, dynamic IR absorbance of the strained sample measured at a wave number, m, can be seen as the combination of two components: a quasistatic [A(m)] and a dynamic one [A˜(m,t)]. ˜ tÞ Aðm; tÞ ¼ AðmÞ þ Aðm;
ð2Þ
with Aˆ(m) being the amplitude and b being the phase loss angle. As the reorientations of the dipole transition moments are directionally dependent, the resulting directional absorbances represent the time-dependent reorientations of the submolecular groups, which are strongly influenced by the intermolecular and intramolecular interactions. The phase difference is due to the rate-dependent nature of the reorientation process of the different submolecular groups. As a result of this, the rheo-optical response can be expressed by the rate-independent ‘‘in-phase’’ and the rate-dependent ‘‘out-of-phase’’ portion of the response, the first representing the storage modulus and the second the loss modulus of the sample. The storage modulus stands for the ability of a polymer to elastically store the absorbed mechanical energy as potential energy, whereas the loss modulus represents the ability of the material to dissipate the absorbed energy. The dynamic response given in Eq. (2) can therefore be expressed as the sum of two terms, which are orthogonal to each other: ˜ tÞ ¼ AVðmÞ sin xt þ AWðmÞcos xt Aðm;
ð3Þ
AV(m) represents the dynamic responses that are in-phase with respect to the applied external perturbation. AW(m) represents the dynamic responses that are 90j out-of-phase with the applied perturbation (cp. Fig. 3). The in-phase spectrum is derived from reorientations of the dipole transition moments occurring simultaneously with the applied strain. The response of the in-phase spectrum is proportional to the applied perturbation. The out-of-phase (quadrature) spectrum shows signals of submolecular constituents which are reorienting with a phase delay of p/2—that means perpendicular to the applied perturbation.
ð1Þ
The dynamic response obtained as a dynamic variation of the IR signals [A˜(m,t)] can be expressed in terms of two parameters. The first is a phenomenological coefficient relating the amplitude of the oscillatory strain to the IR response [Aˆ(m)] and the second representing the phase loss angle (b) between the strain and the IR response. As the sinusoidal external perturbation is applied at a fixed fre-
Figure 3 Connection of magnitude and phase spectra to inphase and out-of-phase spectra.
2D FT-IR Spectroscopy Applied to Cellulose and Paper
163
The in-phase and out-of-phase spectra can be expressed as follows: ˆ AVðmÞ ¼ AðmÞcos bðmÞ ð4Þ ˆ AWðmÞ ¼ AðmÞsin bðmÞ The in-phase and out-of-phase spectra are related to the magnitude and phase spectra (see Fig. 3) mathematically as follows: qffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffiffi ˆ AðmÞ ¼ ðAVðmÞ2 þ AWðmÞ2 Þ ð5Þ bðmÞ ¼ arctanðAWðmÞ=AVðmÞÞ An additional method for analyzing the spectra was introduced by the two-dimensional infrared correlation analysis [71–73]. Again, time-resolved detection of IR signals in response to an external perturbation, e.g., mechanical strain, was the basis. In contrast to the former correlation analysis, the dynamic variation of the IR signals was analyzed yielding new spectra which were defined as functions of two independent wave number axes. For a pair of dynamic IR signals measured at two different wave numbers, the dynamic IR cross-correlation functions were defined, giving synchronous and asynchronous spectra. The synchronous correlation intensity characterizes the degree of coherence between the dynamic fluctuations of IR signals measured at two different wave numbers. The asynchronous spectra represent the correla-
tion for changes occurring with 90j phase difference [74]. Peaks located on the 2-D spectra provide information about interactions among the different functional groups associated with the IR bands. A further advantage of this new data handling was that overlapping bands could be resolved. In 2-D IR, the dynamic IR cross-correlation function X(s) is defined for a pair of dynamic IR signals measured at two different wave numbers [A˜(m1,t) and A˜(m2,t)] as, XðsÞ ¼ Uðm1 ; m2 Þcos xt þ Wðm1 ; m2 Þsin xt
ð6Þ
where U(m1,m2) and W(m1,m2) are the real and imaginary components, respectively. The synchronous and asynchronous correlation intensities of the dynamic spectrum are given by: 1 ˆ ˆ Uðm1 ; m2 Þ ¼ Aðm 1 Þ Aðm2 Þcos½bðm1 Þ bðm2 Þ 2 1 ¼ ½AVðm1 Þ AVðm2 Þ þ AWðm1 Þ AWðm2 Þ ð7Þ 2 1 ˆ ˆ Wðm1 ; m2 Þ ¼ Aðm 1 Þ Aðm2 Þsin½bðm1 Þ bðm2 Þ 2 1 ¼ ½AWðm1 Þ AVðm2 Þ AVðm1 Þ AWðm2 Þ ð8Þ 2 Fig. 4 gives an example of a synchronous spectrum in the wave number region 3600–2500 cm1 of an oriented cellulose sheet irradiated with IR light polarized parallel to
Figure 4 Synchronous 2-D FT-IR spectrum of an oriented cellulose sheet irradiated with IR light polarized parallel to the stretching direction. Autopeaks on the diagonal are marked as (.) and cross-peaks as (5).
164
the stretching direction. The 2-D IR correlation spectrum is in fact three-dimensional, with independent wave numbers on the x- and y-axes and the correlation intensities on the zaxis. In a synchronous spectrum, peaks appear for pairs of bands with identical dynamic behavior. The peaks on the diagonal, the so-called autopeaks, indicate which transition dipoles and thus which submolecular components have an orientational response to the applied sinusoidal strain. Since the intensity change of each band is correlated with itself, a series of positive maxima along the diagonal show up. The off-diagonal peaks (cross-peaks) appear whenever the corresponding dipole transition moments reorient inphase (simultaneously) with each other. Therefore a pair of intense cross-peaks indicates the existence of a strong synchronous correlation between the two bands. If the cross-peak appears to be positive in sign, the two corresponding dipole transition moments reorient parallel to each other. Negative peaks appear if the reorientations are mutually perpendicular. Further details of the cellulose spectrum will be discussed under ‘‘Two-Dimensional FTIR Spectroscopy Applied to Cellulose’’ of this chapter. The asynchronous correlation function (an example for the wave number region 3500–3200 cm1 is drawn in Fig. 5) gives information about the degree of independence of reorientational behavior of corresponding dipole transition moments. No peaks appear on the diagonal. Cross-peaks are produced if the transition dipoles reorient out-of-phase with each other, meaning that they are not
Salme´n et al.
synchronized and therefore that a strong chemical interaction is lacking. Functional groups that are located in different chemical environments can exhibit different dynamic responses to the external perturbation. The signs of the cross-peaks give information on the relative rates of the response of the involved dipoles. Fig. 5 gives an example of the asynchronous correlation map of the OH region of an oriented cellulose sheet irradiated with IR light polarized parallel to the stretching direction. The static spectrum consists of a broadband, obviously derived from the overlapping of several bands. This can clearly be observed in the 2-D plot where several different crosspeaks, also with a different sign, appear. Because of the mathematics, equivalent peaks with opposite signs appear on the different sides of the diagonal. A closer discussion of these features for the cellulose bands in question will also follow in ‘‘Two-Dimensional FT-IR Spectroscopy Applied to Cellulose’’ of this chapter. In the years following the development of this 2-D FTIR technique, investigations on several synthetic polymers such as polyurethane [75], polyethylene [70,76], polypropylene [77,78], polymer films and liquid crystals [79], epoxy resins [80,81], polymer blends [82–84], melt crystallized nylon [85], acetylene terminated polyisoimide prepolymer [86], duroquinone [87], and inorganic NaCl crystals [88] have been performed. The method has also successfully been applied to some biological materials, for instance, to study protein conformations in human skin [89], keratin in
Figure 5 Asynchronous 2-D FT-IR spectrum of an oriented cellulose sheet irradiated with IR light polarized parallel to the stretching direction. Cross-peaks are marked as (0).
2D FT-IR Spectroscopy Applied to Cellulose and Paper
165
human hair [89,90], fibroin in silk [91], and arabinoxylans [92,93]. The technique was introduced to cellulose research by Hinterstoisser and Salme´n [56–58]. A˚kerholm and Salme´n [59,60] extended the investigations to the wood polymer network to determine which wood polymers were connected to each other and the nature of the interactions. Furthermore, the first studies on pulps were carried out [61].
III. TWO-DIMENSIONAL FOURIER TRANSFORM INFRARED SPECTROSCOPY APPLIED TO CELLULOSE A. Orientation Aspects In dynamic IR spectroscopy, thin films or sheets of a material are stretched. Even with a film of random polymer chain orientation, the small static and dynamic strains put on the sample will shift the random distribution toward a small orientation in the direction of the stretch. This orientation, together with the fact that both the dipoles and the polarized light have a direction, means that the spectral response to the straining will differ in different polarization modes. With a preoriented sample, this difference will be enhanced. The effects of sample orientation on the spectral result of 2-D FT-IR measurements have been studied for isotactic polypropylene samples of different orientation [78]. It was found that for this material, the spectral result depended strongly on the pretreatment of the sample, as well as on the polarization of the infrared radiation used. The spectral features occurring in dynamic FT-IR spectra originate from absorption changes, frequency shifts, and changes in band shape as a result of the applied dynamic strain of the samples. These stress-induced changes have been shown to vary with morphological, thermal, and stress history of the samples. With an oriented film or sheet, the specimen may also be stretched in different directions. Such effects are illustrated in Fig. 6, where the dynamic in-phase spectra for spruce cellulose sheets with different fiber orientations are shown for both 0j polarization and 90j polarization [56]. Comparing the spectra from the different orientations reveals no great difference in band positions between them. The main effects observed for the different fiber directions were the differences in relative intensity between absorption bands. For these cellulose samples, it can be seen that the intensity of the peak for the nonoriented sample is always in-between the intensities of the other two loading modes. There is a strong correlation between the deformation of the cellulose skeleton including the glycosidic bond, the band at 1165/1169 cm1, and the band at 1435 cm1. This can be seen as the peak at 1435 cm1 having the same intensity for all different fiber orientations after normalization of the spectra at 1165/1169 cm1 (skeletal stretching vibrations including the C–O–C bridge stretching). The intensity of the O3–H. . .O5V intramolecular hydrogen vibration is the highest in both the 90j (3332 cm1) and 0j (3329 cm1) polarization modes for the sheet loaded perpendicular to the fiber axis and the lowest for the sheet
Figure 6 Dynamic in-phase FT-IR spectra showing the result of a sheet stretched parallel to the fiber axis, perpendicular to the fiber axis, as well as a non-oriented sheet during 0j (upper spectra) and 90j (lower spectra) polarization modes.
loaded parallel to the fiber axis and is related to the normalization at 1165 and 1169 cm1, respectively. In the case of the perpendicular orientation, there are few cellulose chains oriented in the stretching direction, capable of taking up the load. This load situation results in a low dynamic intensity of the skeletal vibration/C–O–C band. Thus in this case, the overall deformation by bending and shearing of the fibers would show up as a larger change in the O3H. . .O5V intramolecular hydrogen bond deformation. Thus when it comes to a general characterization of the strain distribution within cellulose in a fiber network material like paper, the fiber direction toward the straining direction is not the most important factor in the experimental arrangement for dynamic FT-IR studies since the same peaks for cellulose appeared for all the fiber directions examined. The highest resolution has, though, been obtained using oriented samples mounted so that the stretch is applied in parallel to the fiber direction. In Fig. 7, the dynamic in-phase spectra of spruce cellulose fiber sheets stretched parallel to the fiber direction for light polarized at 0j and 90j to the strain direction [56] are shown. The dynamic spectra recorded at 0j polarization are dominated by changes in vibrations aligned parallel to the straining direction, while spectra recorded at 90j polarization are dominated by perpendicularly aligned vibrations. In general, more peaks appear in the in-phase spectra of the 90j polarization than at 0j, both in the OH region and in the fingerprint region. For both polarizations, the most intense
Salme´n et al.
166
Figure 7 Dynamic in-phase (thick line) and out-of-phase (thin line) FT-IR spectra of cellulose. The fibers of the cellulose sheets were oriented parallel to the stretching direction. The polarization plane of the incident beam was 0j (upper spectra) and 90j (lower spectra) to the strain direction. The most intense bands are marked.
peaks are found between 1200 and 1050 cm1 (CO, CC, and skeletal stretching vibrations). At 0j polarization to the direction of the straining, the two most intense peaks are at 1169 cm1, corresponding to skeletal stretching vibrations including the C–O–C bridge stretching [24,94], and at 3329 cm1, corresponding to the O3H. . .O5V intramolecular hydrogen vibration [6,95,96]. In the 90j experiment, the 1064 cm1 band, in the CO valence vibration region, is the most intense peak. In this polarization mode, there are also peaks for skeletal stretching including the C–O–C stretching, positioned at 1165 cm1, and for the O3–H. . .O5V intramolecular hydrogen vibration at 3332 cm1. Between 1200 and 1500 cm1, CH2 deformation vibrations and COH in-plane bending motions are expected. More signals appear in the 90j than in the 0j polarization experiment for this area, but the intensity is less than that for the lower wave numbers. As the peak at 1462 cm1, probably from a CH2 bending vibration [97], represents an orthogonal vibration in relation to the backbone, its appearance in only the 90j polarization experiment is anticipated.
B. Load Distribution In understanding the strength development of polymeric material and the way this is affected under various con-
ditions, the understanding of how different entities of the molecule contribute is essential. This applies in particular to a system such as that of cellulose in which there are possibilities for hydrogen bonding in several different positions. In fact, cellulose is a very highly coupled system in terms of IR vibrations. This is demonstrated via the synchronous 2-D FT-IR spectrum in Fig. 8. As an example, the close correlation between the O3–H. . .O5V intramolecular hydrogen and a skeletal stretching band can be observed in the 2-D spectrum as a significant cross-peak between 3329 and 1169 cm1, the latter often assigned in the literature to the COC stretching [16,97,98]. This band, though, is not a real local mode vibration and therefore cannot be solely stated to be a C–O–C stretching mode, as the glycosidic linkage is part of a whole sequence of eight coplanar CC or CO bonds and these bonds are very highly coupled in their vibrations. The O3 bond, which is the last in the sequence, is precisely the one that is involved in the intramolecular O3H. . .O5V hydrogen bond [94]. The relatively high intensity of the O3–H. . .O5V intramolecular hydrogen vibration, the high intensity of the skeletal vibrations including the C–O–C bridge stretching, and the high intensity of the C–O and ring stretching in general (Fig. 7) all point to their importance in the loading of the cellulose chain. This fact, in combination with the close coupling observed in the 2-D FT-IR spectrum (Fig. 8) [56], supports the calculations of Tashiro and Kobayashi [97], who found that the strain energy in cellulose is mainly distributed via deformation of the glucose rings (f30%), bending of the ether linkages connecting the adjacent rings (f20%), and deformation of O3H. . .O5V hydrogen bonds (f20%). In this respect, the O2VH. . .O6 intramolecular hydrogen bond seems to play a minor role.
C. Hydrogen Bonding 1. General Remarks Hydrogen bonds are of special interest when dealing with macromolecules, particularly biomacromolecules. The reason is evident: hydrogen bonds are known to be the most important cohesive forces involved in the organization of the three-dimensional structure and the mode of recognition and association of biological molecules. Furthermore, they are known to be stronger and more directional than van der Waals forces [99]. It was during the 1930s that hydrogen bonds were introduced as an important principle in structural chemistry [100,101]. It was then that the interest in research into this incredibly important issue that hydrogen in special cases has the ability to function as a ‘‘bridge atom’’—a function being of basic importance for life—began. The strength of hydrogen bonds ranges from something close to that of covalent bonds down to a primarily electrostatic interaction, depending on the other partners involved. On the one hand, the hydrogen atom within the functional group might be covalently bound to a more electronegative atom. On the other hand, the hydrogen atom might face as its nearest neighbor another electro-
2D FT-IR Spectroscopy Applied to Cellulose and Paper
167
Figure 8 Synchronous 2-D FT-IR spectrum of oriented cellulose sheets stretched parallel to the fiber orientation, irradiated with IR light polarized parallel to the stretching direction and the fiber direction (0j polarization mode). The cross-peaks can be seen off the diagonal. The cross-peak between the band of the COC and the O3H. . .O5V hydrogen bond is marked.
negative atom. This belongs to another functional group which serves as electronegative acceptor within the hydrogen bonding. As the electron of the hydrogen atom is used for the closure of the covalent bond to the more electronegative atom, the hydrogen becomes more or less descreened. This results in a dipole with a positive charge at the H-end of the linkage. If the nearest neighbor is carrying excess electron density, a hydrogen bond to this neighbor is built. The strength of the hydrogen bond depends mainly on the electron affinity of the partners involved. From this point of view, it is easy to understand that a variety of hydrogen bonds exist. These vary both in bond energy and in their structural features. Very strong hydrogen bonds such as that in FH. . .F and OH. . .O are of minor importance in biological systems. More important in these are the ‘‘normal’’ or ‘‘weak’’ hydrogen bonds. These are often two, three, or four centered bonds, with a bond length ranging from 0.15 to 0.3 nm. They are weakly directional, the bond energy is lower than 20 kJ/mol, and the IR vibration frequencies are found above 2000 cm1 [99]. Hydrogen bonds lead to a remarkable red shift (shift toward longer wavelengths) of the OH stretching vibration bands in IR spectra, as the bonding between the electronegative oxygen and the hydrogen atom is weakened through the bridge building. The OH stretching vibration frequency, for example, of
an alcohol diluted in CCl4, or CS2, for instance, appears at about 3600 cm1. The corresponding OH stretching vibration of a pure, and therefore very much associated, alcohol is a broadband around 3300 cm1 [102]. Weak hydrogen bonds are long-range interactions, falling off with r1. The first neighbor hydrogen bond interactions are still significant at distances as great as 0.35 nm from the hydrogen atom. Hydrogen bonds, therefore, appear to have group properties. This means that they depend not only on their nearest neighbor atoms involved in the bridge building, but also on the sequential nature of the total pattern of bonding. In general, the stretching and bending force constants of hydrogen bonds are about 15 times smaller than for covalent bonds. However, bond length and angles depend a lot on the chemical environment. Hydrogen bonds can be easily deformed by other intermolecular interactions, such as other hydrogen bonds or van der Waals forces [99]. Intramolecular hydrogen bonds differ from intermolecular ones as they are not affected by solvents because they are less accessible [28,102]. Consequently, hydrogen bonds are a complex issue to study. Differences particularly in bond length, energy, and angles imply that they also differ in their vibrational behavior, making IR spectroscopy a useful tool for such investigations.
168
2. Hydrogen Bonding in Cellulose There is no question about the general concept that cellulose is made up of glucose molecules forming poly-h(1,4)D-glucose chains. On the other hand, many researchers have put much effort into answering questions relating to its three-dimensional structure, questions undoubtedly concerned with hydrogen bonds, and the matter is not yet resolved. In fact, intramolecular as well as intermolecular hydrogen bonds play a major role in the interactions within and between the cellulose molecules and, therefore, also influence the strength properties of the cellulosic material. Intramolecular hydrogen bonds have an important stabilizing function within cellulose chains. The intermolecular hydrogen bonds are also of importance as they play a key role in the formation of crystalline structures and the association of microfibrils. The physical properties of dry cellulose, for example, the fiber-to-fiber linkage in paper, are mainly a function of the OH groups and their ability to build hydrogen bonds. In dry cellulose, practically all OH groups are involved to some extent in hydrogen bonding. The proton donor group is an OH group bonded to another hydroxyl or oxygen group, functioning as proton acceptor. Some of these hydrogen bonds can be destroyed by water leading to new hydrogen bond formation between the OH or O groups of the cellulose and the water molecules. The accessibility of different hydrogen bonds is selective in character, the intramolecular bonds being more resistant than the intermolecular ones [28]. Studies of hydrogen bonding are an intrinsic part of cellulose research. Since the 1950s, IR spectroscopy has been one of the favored tools for investigating hydrogen bonds, although the broadband around 3000–3700 cm1 causes difficulties in spectral interpretation because it includes all the specific OH stretching vibration bands of interest in one large peak. Several attempts have been made to unravel this ‘‘hump’’ by using deuterium exchange (for example, Refs. [11,21,103]), as well as mathematical processing such as deconvolution and differentiation [34,95]. As investigations proceeded over the years, specific frequencies were assigned to different hydrogen bonds. This became even more important with the discovery that there existed different allomorphs of native cellulose (cp. ‘‘Crystal Structure’’), which opened up further discussions relating to hydrogen bonding. In the generally accepted structure of native cellulose (Fig. 9), intramolecular hydrogen bonds of types O3H. . .O5V and O2VH. . .O6 are present on both sides of the chain [104]. This is related to a nearly trans gauche (tg) orientation of the hydroxymethyl group [105]. The bond length of the O3H. . .O5V hydrogen bond is reported to be 0.275 nm and the length of the O2VH. . .O6 is reported to be 0.287 nm. An intermolecular hydrogen bond, O6H. . .O3, is formed with a bond length estimated to be 0.279 nm [104,105]. It is generally known and accepted that these hydrogen bonds play an important role in determining the conformational and mechanical properties of cellulosic materials [19,55,104–106]. However, no satisfactory verifi-
Salme´n et al.
Figure 9 Schematic drawing of cellulose molecules including the hydrogen bonds (----): intramolecular hydrogen bonds O3H. . .O5V and O2VH. . .O6; intermolecular hydrogen bond O6H. . .O3.
cation of the predicted vibrational energies of the different bondings is at hand. The dynamic 2-D FT-IR technique has, in this respect, been found useful in providing answers to the remaining questions relating to hydrogen bonding [56–58]. Fig. 10 shows an example of the OH stretching vibration region in both static and dynamic 2-D FT-IR spectra of native spruce cellulose. These spectra were produced from oriented sheets made of a spruce dissolving pulp. Comparing the dynamic in-phase and out-of-phase IR spectra, the first fact to emerge is that the response of the out-of-phase spectrum is two to three times less intense than that of the in-phase spectrum. This indicates that the dynamic behavior of the cellulose is nearly exclusively elastic. The second and even more obvious feature is that the in-phase IR spectra consist of different distinct bands, while the static spectra consist of an unstructured broadband. The higher resolution provided by the dynamic measurement allows experimental visualization of the bands belonging to different dipole transition moments. There are also differences between the spectra measured in the parallel polarization mode and those measured in the perpendicular mode. The main band in the 0j polarization mode experiment appears, in fact, as a split, or a so-called bipolar, band. This indicates that the transition dipole moments of the components involved reorient in different directions with respect to the polarization axis when subjected to the oscillatory strain. One average dipole is moving toward the polarization axis, which is in this case parallel to the strain axis, and the other away from it. The dominating signal is placed at 3329 cm1 with an opposite peak at 3372 cm1. A bipolar dynamic band has its ‘‘fundamental’’ energy in-between the two bands. Further details are examined and discussed in connection with 2-D correlation spectra. In Fig. 11, the synchronous correlation spectrum of the OH region of spruce cellulose is shown. The spectrum is symmetric with respect to the diagonal line as the synchronous correlation intensities characterize the degree of coherence between the dynamic fluctuations of IR signals measured at two different wave numbers. As mentioned above, the autopeaks indicate which functional groups change dynamically as a result of the applied sinusoidal strain.
2D FT-IR Spectroscopy Applied to Cellulose and Paper
169
Figure 10 OH-stretching vibration region of FT-IR spectra: static spectra (----), in-phase and out-of-phase dynamic spectra of native spruce cellulose stretched parallel to fiber orientation: (A) light polarized parallel and (B) light polarized perpendicular to the stretching direction.
The observed autopeaks in the synchronous 2-D spectrum in the OH range thus represent the perturbationinduced local reorientation of the hydrogen bonds. The main peaks are at 3329, 3372, and 3472 cm1. As the cellulose molecule reacts quite elastically, the peaks observed are equal to the ones observed in the in-phase spectra. The synchronous plot of the oriented sheets shows strong positive cross-peaks, correlating the main maxima with each other. Obviously, these dipole transition moments reorient in phase with each other, showing a high degree of coupling. Negative cross-peaks (shaded in the figure) between 3329 cm1 and the other peaks are clearly evident. The appearance of negative cross-peaks indicates that the reorientation direction of the one transition dipole moment is orthogonal to that of the other. Therefore it can be concluded that the transition dipole moment of the 3329 cm1 band is perpendicular to that of the 3372 and 3472 cm1 ones. It is therefore clear that although the two sets of absorption bands are synchronized to each other, they must have different origins. According to the literature, the frequencies for the O3H. . .O5V intramolecular hydrogen bond can be found between 3340 and 3375 cm1 [6,28,97]—the peaks of the in-phase spectra are almost within this wave number region. Examining again the in-phase spectra shown in Fig. 10, it can be seen that in the 90j polarization mode (Fig. 10B), a corresponding peak appears at 3332 cm1, but this one is not split. A band at 3375 cm1 is, however, unidirectional with the 3332 cm1 in the 90j polarization mode. It appears as well in the region predicted for the O3H. . .O5V intramolecular hydrogen bond leading to the question of whether a bifurcated hydrogen bond might exist, as Atalla [19,94] has suggested for h-methylcellobioside. In the 0j polarization experiments (Fig. 10A), transition dipole
moments reorienting in the stretching direction give a stronger contribution to the spectrum, and it is the hydrogen bonds involved that are more likely to be stretched and changed in energy during straining. The high intensity of the O3H. . .O5V intramolecular hydrogen bond vibration, and its domination in the 0j polarization mode, clearly indicate its importance in the loading of the cellulose chain as a kind of ‘‘second bridge’’ between adjacent glucose molecules beneath the main, covalent COC bridge. As the intramolecular hydrogen bonds O3H. . .O5V and O2VH. . .O6 are expected to be stabilizers in the cellu-
Figure 11 Synchronous 2-D FT-IR spectrum of the OHstretching vibration region of native spruce cellulose stretched parallel to the fiber orientation and irradiated with light polarized parallel to the stretching direction. Negative cross-peaks are shown shaded.
170
Salme´n et al.
lose molecule, they should both be found as well-recognizable bands in the dynamic spectra. As the bond length of the O2VH. . .O6 intramolecular hydrogen bond [104,105] is longer than that of the O3H. . .O5V hydrogen bond, the associated band will appear at a higher frequency, namely, between 3410 and 3460 cm1 [6,107]. Only small bands were found in this range in the 2-D spectrum, emphasizing that the O2VH. . .O6 intramolecular hydrogen bond obviously plays a minor role in the load distribution [56]. In general, it is clear that more signals appear in the 90j polarization mode. For well-ordered samples of spruce cellulose, the band at 3267 cm1 is the most intense in this polarization direction. There is also a shoulder in the inphase spectrum at 3232 cm1. These two bands are close to the characteristic cellulose I h and cellulose Ia bands assigned to 3270 and 3240 cm1, respectively [17]. Both of them are in the suggested wave number area for the O6H. . .O3 intermolecular hydrogen bond between 3230 and 3310 cm1 [6,11,17,95]. This assignment might be questioned as the O. . .O distance is slightly greater than that of O3H. . .O5V intramolecular bond, and therefore the band is expected to occur at higher frequencies [94], but according to Gardner and Blackwell [104], as well as by Okamura [105], the distance is quite close to the O3H. . .O5V bond length. In the 90j polarization mode, the response in the dynamic spectrum is preferentially from orthogonal vibrations in relation to the stretching and the main direction of the cellulose chains. Hence the intermolecular hydrogen bonds, connecting adjacent molecular chains, are likely to provide the main signal in the 90j polarization mode. The allomorph-characteristic bands of cellulose I can also be seen in the 0j in-phase spectrum, but they are not the main bands in this case. The asynchronous spectrum of the orientated spruce cellulose samples irradiated with IR light polarized parallel to the stretching and to the fiber orientation is shown in
Fig. 12. Several cross-peaks can be found on the plot. Two cross-peaks near the diagonal establish a correlation square at 3332 cm1 giving two distinguishable bands at 3332 and 3314 cm1. Another cross-peak is found at 3362 cm1. Only nonsynchronized responses appear in the asynchronous spectrum. There is thus no cross-peak between bands at 3372 and 3329 cm1, again underlining a high coupling of these two. Specific assignments of the different new bands cannot be given at this stage. Figs. 13 and 14 show the 2-D plots for the experiments carried out on the oriented sheets in the 90j polarization mode. In the synchronous spectrum (Fig. 13), again, autopeaks appear (3267, 3332, 3372, and 3440 cm1)
Figure 12 Asynchronous 2-D FT-IR spectrum of oriented cellulose sheets, IR light polarized parallel to stretching and to fiber orientation.
Figure 14 Asynchronous 2-D FT-IR spectrum of oriented cellulose sheets. IR light polarized perpendicular to the stretching and to the fiber orientation.
Figure 13 Synchronous 2-D FT-IR spectrum of oriented cellulose sheets. IR light polarized perpendicular to the stretching and to fiber orientation.
2D FT-IR Spectroscopy Applied to Cellulose and Paper
171
coupled to one another via positive cross-peaks. The reorientation directions of the dipole transition moments are obviously the same for these bands. Interestingly, in the asynchronous spectrum (Fig. 14), a cross-peak is found between the bands of 3267 and 3232 cm1, which is between the bands assigned to cellulose Ih and Ia, respectively, clearly distinguishing these two signals.
D. Crystal Structure Native cellulose is a composite of two different crystalline forms, cellulose Ia and cellulose Ih [108]. These two allomorphs are suggested to differ in their secondary structures which is in the conformation around the glucosidic linkage and the C5C6 bond, the hydrogen bonding patterns, or the molecular packing [54]. Although differences in IR spectra of different native celluloses were revealed almost 50 years ago [109], the highly overlapping bands in the IR spectra of biopolymers have meant that the possibilities of studying such structural differences using conventional IR spectroscopy have been reduced. The 2-D IR technique is, however, sensitive to the secondary structure since differences in the molecular environment for a transition dipole result in different responses when the polymers are dynamically strained during the experiment. This opens up new possibilities for IR spectroscopy because 2-D IR spectroscopy is not only sensitive to chemical composition, but also to structural conformations such as the secondary structure of the polymers. During pulping of wood, the fibers are exposed to high temperatures under alkaline or acidic conditions. The
Figure 16 Dynamic FT-IR intensity of 3240 cm1 plotted against relative cellulose Ia content in cellulose mixtures of cotton linters and a Cladophora cellulose.
pulping processes not only dissolve the lignin from the wood structure, but also affect the hemicellulose and cellulose structures. Such differences in cellulose structure between differently pulped fibers have been demonstrated by NMR spectroscopy [110–113]. FT-IR spectroscopy has also been used to determine the allomorphic composition of cellulose I from different origins. Sassi et al. [114] used the deconvoluted bands of the OH stretching vibrations, whereas Imai and Sugiyama [49] determined the ratio of the
Figure 15 Comparison of dynamic and static FT-IR spectra of one cellulose mixture for two areas where characteristic peaks of cellulose Ia and cellulose Ih are to be found. Thick line=static spectrum and thin line=dynamic spectrum.
172
Figure 17 Dynamic FT-IR intensity of 756 cm1 plotted against relative cellulose Ia content of cellulose mixtures of cotton linters and a Cladophora cellulose.
absorption coefficients between 750 and 710 cm1. Yamamoto et al. [115] also used the 750 and 710 cm1 peaks, but made line–shape analyses of the spectra and then correlated the ratios to the mass fraction determined by 13C NMR. All these studies were, however, carried out on highly ordered materials such as Cladophora, Valonia, and bacterial celluloses, whose FT-IR spectra are higher in resolution compared to the spectra of wood celluloses. With the 2-D FT-IR method, characteristic IR peaks of cellulose Ia and cellulose Ih may also be studied in pulp samples [61,116]. The higher resolution of the dynamic compared to the static IR spectrum with regard to the characteristic peaks of celluloses Ia and Ih [17] is shown in Fig. 15 for a mixture of two different native celluloses, a cotton linters Ih-rich cellulose and a Cladophora (algae) Ia-rich cellulose.
Salme´n et al.
The bands characteristic of cellulose Ia and cellulose Ih in the OH region are reported to be found at 3240 and 3270 cm1, respectively [17]. These bands are marked in the static spectrum of Fig. 14. It can be seen that in the dynamic in-phase spectrum, the peak maxima differ from these. This is a result of the change in the energy of the vibration as a result of the straining of the polymer (the so-called split/ bipolar dynamic peaks [78]). The peak-to-valley intensity of the characteristic cellulose Ia peak at about 3240 cm1 may be used for quantitative purposes as illustrated in Fig. 16 for mixtures of pure celluloses, cotton linters, and a Cladophora cellulose. The correlation was, however, linear only for the mixed samples (18–42% cellulose Ia). For chemical pulps, the resolution in this region compared to the pure celluloses is too low for quantitative evaluation. In the low wave number region, the characteristic Ia peak (750 cm1) is also slightly shifted in the dynamic spectrum (Fig. 15, right). The static peak characteristic of cellulose Ih at 710 cm1 could also be found in the dynamic spectrum, and additionally, the dynamic spectrum contains a third peak at 725 cm1. In this wave number region, 800–700 cm1 (OH out-of-plane bending [19]), a correlation to the allomorphic composition is only linear for the 710 cm1 peak. The characteristic cellulose Ia peak at 756 cm1 only shows a linear correlation between peak intensity and allomorphic composition for cellulose Ih-rich samples. When cellulose Ia contents are above about 30%, some kind of saturation point is reached (Fig. 17). The intensity of the peak at 725 cm1, which only appears in the dynamic spectrum and not in the static one, is independent of cellulose allomorphic composition pointing to its relationship to some feature other than the allomorphic composition or the crystallinity in general (Fig. 18). The peak at about 710 cm1 (characteristic of cellulose Ih) has a linear correlation with the relative cellulose Ih content as seen in Fig. 19. This correlation was used as a
Figure 18 Dynamic FT-IR intensity of 725 cm1 plotted against relative cellulose Ia content of cellulose mixtures of cotton linters and a Cladophora cellulose.
2D FT-IR Spectroscopy Applied to Cellulose and Paper
173
Figure 19 Dynamic FT-IR intensity of 710 cm1 plotted against relative cellulose Ih content of cellulose mixtures of cotton linters and a Cladophora cellulose.
basis for estimating cellulose allomorphic composition in pulps [116]. Moreover, this peak also shifts linearly in wave number position from 706 cm1 in the pure cotton linters sample to 714 cm1 in the pure Cladophora sample. The different positions of this band have also been reported for other native celluloses [17]. For wood pulps, the dominating peak in this low-wave number region is the 725-cm1 peak, indicating that structural differences exist in relation to cotton and Cladophora
cellulose. However, the 710-cm1 peak also differs in intensity between different chemical pulps (Fig. 20). The 710-cm1 peak may therefore be used together with the correlation from the cotton/Cladophora mixtures (Fig. 19) to estimate the relative cellulose Ih content of these chemical pulps (Table 1). As seen from Table 1, the birch kraft pulp has a higher content of cellulose Ih than the two corresponding softwood kraft pulps studied. This is most likely related to the fact that birch wood is more enriched in the cellulose Ih form, while softwoods are more enriched in the cellulose Ia form [117]. The holocellulose and the acid sulfite pulp have the lowest amounts of cellulose Ih, whereas the dissolving pulp has the highest amount. The higher amount of cellulose Ih in chemical pulps compared to holocellulose has also been demonstrated with NMR measurements [111,112]. The reason for the altered allomorphic composition is that the monoclinic cellulose Ih form is more thermodynamically stable, and therefore
Table 1 Estimations of relative content of cellulose Ih in pulps Pulp sample
Figure 20 Dynamic in-phase FT-IR spectra at 0j polarization for different chemical pulps. The spectra are plotted at different offsets.
Dissolving pulp Bleached softwood Kraft Softwood kraft liner Birch kraft Acid sulfite pulp Holocellulose
Estimated relative content of cellulose Ih (%) 79 (F2.0) 49 50 54 41 43
(F2.8) (F5.7) (F0.9) (F0.9) (F0.4)
Numbers in parentheses are the standard deviations based on three measurements.
174
Salme´n et al.
conversion from the triclinic cellulose Ia to cellulose Ih occurs at the high temperature and alkalinity of the kraft process. The acid sulfite pulping process does not appear to affect the allomorphic conversion in the same way, as also revealed by NMR [113]. The reason for this could be that this transformation is affected both by the temperature as well as the medium, where an alkaline medium is favorable for the transformation [46]. Another factor worth considering is the structural hindrance to transformation that the lignin might provide during pulping. In acid sulfite pulping, the lignin is in a rather unswelled state and softens subsequently, in contrast to its behavior in the alkaline kraft process [118]. It is suggested that this reduces the diffusion rates in the fiber wall and might also reduce the chance for cellulose to structurally rearrange.
IV. TWO-DIMENSIONAL FOURIER TRANSFORM INFRARED SPECTROSCOPY APPLIED TO PULPS A. Hemicellulose Interaction Two-dimensional IR spectroscopy is particularly useful for studies of interactions between different polymers in composite materials. Although there have been numerous studies on synthetic composites (see ‘‘Infrared Spectroscopy for Wood and Cellulose Research’’ of this chapter), only a few studies have dealt with interactions within composites of biopolymers, such as wet onion cell walls [119], composites of Acetobacter cellulose [93], and different pulp fibers [59–61]. For a native composite such as the wood cell wall, such studies of these interactions could contribute much toward the understanding of the ultrastructural arrangement of the polymers within this biologically constructed material.
Figure 21 Weights from partial least squares (PLS) analyses of extracted holocelluloses. Positive peaks show high contribution from the polymer to the absorption in this area.
Figure 22 Static FT-IR spectrum of a spruce holocellulose. Characteristic vibration bands from the different polysaccharides in wood pulps are marked in the diagram.
1. Characteristic Vibrations In using 2-D IR spectroscopy to study interactions between polymers in a composite, it is a prerequisite that absorption peaks for the different polymers are distinguishable. This was, in fact, thought to be an obstacle in the interpretation of dynamic spectra in such a study of polysaccharide interactions in onion cell walls [119]. Since the different polysaccharides in the wood cell wall are all built up with sugar units, they also have very similar IR spectra. However, the glucomannan (or more correctly, O-acetyl-galactoglucomannan) has characteristic vibrations due to the equatorially aligned hydrogen in the mannose unit. These vibrations can be found at 810 and 870 cm1. Furthermore, it is the vibration characteristics of carboxylic acids (1735, 1600, and 1245 cm1) from the 4-O-methyl-a-D-glucopyranosyl uronic acid side group of xylan [arabino-(4-Omethylglucurono)xylan in softwoods and O-acetyl-(4-Omethylglucurono)xylan in hardwoods] that distinguish the xylan spectrum from the cellulose spectrum. These characteristics have been demonstrated in a multivariate data analysis on alkali-extracted holocelluloses [59] (Fig. 21). It is difficult to spectrally distinguish between cellulose and glucomannan. A high correlation between the cellulose content in holocelluloses and the bands at 1110, 1315, 1335, and 1430 cm1 has, though, been demonstrated. These bands are sensitive to cellulose crystallinity [27,120] and are therefore more distinct in the spectrum of the more ordered cellulose compared to glucomannan. In Fig. 22, the characteristic vibration bands of the three main polysaccharides within wood pulps are marked in a static FT-IR spectrum of a spruce holocellulose sample. 2. Holocellulose The production of holocellulose by treatment with sodium chlorite under acidic conditions is known to remove the lignin without causing major changes to the native structure of the wood cell wall. Therefore such a sample can be
2D FT-IR Spectroscopy Applied to Cellulose and Paper
Figure 23 Dynamic in-phase (thin line) and out-of-phase (thick line) FT-IR spectra of spruce holocellulose sheets strained in the fiber direction. The spectra are recorded at 90j polarization.
used as a reference for the polymer interactions in the native wood fiber if lignin-free samples are required. In Fig. 23, the two components of the dynamic spectrum of a spruce holocellulose are shown [59]. These measurements have been performed at room temperature in dry air. The weak out-of-phase (viscous) signal points to a very elastic response of the sample under these condi-
175
Figure 25 Model of the cell wall structure of a latewood softwood fiber (tracheid). The lines in the different cell wall layers represent the organization of the cellulose fibrils in the different layers. Observe the dominance of the S2 layer with the fibrils aligned almost parallel to the fiber axis. (From Ref. 138.)
tions. The glass transition of the dry wood polysaccharides firstly occurs at temperatures over 180jC, implying that they are all in their glassy state at room temperature under dry conditions [118]. Under these conditions, it is in the inphase dynamic spectrum that the information will be found since the out-of-phase spectrum mainly consists of noise. Therefore in the following discussion, concerning holocel-
Figure 24 Comparison of dynamic in-phase FT-IR spectra at 0j polarization for a spruce cellulose (dissolving pulp free of hemicelluloses) (thin line) and a holocellulose (cellulose with 33% hemicelluloses) (thick line). The sheets are strained in the fiber direction.
176
Salme´n et al.
Figure 26 Comparison of dynamic in-phase FT-IR spectra at 90j polarization for spruce cellulose (thin line) and holocellulose (thick line). The sheets are strained in the fiber direction.
Figure 27 Comparison of dynamic in-phase FT-IR spectra at 90j polarization for spruce cellulose (thin line) and holocellulose (thick line). Characteristic vibrations of glucomannan due to the orthogonal directed hydrogen of the mannose ring are marked at 810 and 870 cm1 in the figure.
lulose and chemical pulps, only the in-phase spectra (elastic response) are shown in the figures. The dominance of cellulose fibrils for the load-carrying ability in pulp fibers is clearly evident from the comparison of the dynamic in-phase IR spectra in 0j polarization of a spruce cellulose (dissolving pulp with >98% cellulose) and a spruce holocellulose containing 33% hemicellulose as seen in Fig. 24. These fiber sheets are strained in the fiber direction. Although the holocellulose is composed of over one-third hemicellulose, the dynamic spectrum looks very similar to that of the pure cellulose. There are no dynamic peaks in the holocellulose spectrum characteristic of xylan or glucomannan, which, however, can be found in the static IR spectrum (Fig. 22). Since 2-D IR spectroscopy only shows changes in intensity as an effect of external perturbation (straining), only the polymers involved in the stress transfer will contribute to the dynamic spectrum. The structure of the wood cell wall is built up of different layers (Fig. 25). In the dominant S2 layer, which makes up 75–85% of the cell wall, the cellulose is arranged in fibrils oriented mainly in the direction of the fiber axis [121]. These cellulose fibrils, which are embedded in a matrix of lignin and hemicellulose, act as reinforcement and therefore take most of the load in the fiber direction. It is therefore not surprising that there are only the dynamic signals from cellulose in the holocellulose spectrum. The differences seen between the two in-phase spectra in Fig. 24 are mainly related to the differences in cellulose structure originating from changes occurring during pulping as discussed in ‘‘Crystal Structure.’’
2D FT-IR Spectroscopy Applied to Cellulose and Paper
Figure 28 An off-diagonal part of the synchronous 2D spectrum at 90j polarization of the spruce holocellulose. Characteristic peaks of cellulose and glucomannan are listed beside the figure and cross-peaks between the two polymers are marked with arrows in the figure.
If similar sheets of fibers of spruce cellulose and spruce holocellulose are studied in the same loading mode, but with 90j polarization instead, the spectra look different (Fig. 26). In this case, vibrations oriented perpendicular to the straining direction are more enhanced. In the 90j polarization spectra, differences between the holocellulose and cellulose can be seen between 800 and 900 cm1 (enhancement in Fig. 27). As mentioned earlier, this area contains absorption peaks characteristic of glucomannan. The appearance of dynamic peaks at 810 and 870 cm1 shows that glucomannan is also taking part in the load transfer in the fiber direction. The fact that they appear at
177
90j and not at 0j polarization is due to the fact that the characteristic vibrations of glucomannan are oriented perpendicular to the backbone of the polymer chain, and the fact that the backbone of glucomannan is oriented parallel to the cellulose chains [59]. As described earlier, the synchronous and asynchronous 2-D spectra are useful for studying interactions between the polymers in a composite. In Fig. 28, an offdiagonal area (different wave numbers on x- and y-axes) of the synchronous 2-D spectrum from a 90j polarization measurement of a spruce holocellulose is shown. The area chosen is where characteristic bands of cellulose and glucomannan appear. The off-diagonal cross-peaks represent similar time-dependent movements of the molecular groups. The appearance of cross-peaks between all the characteristic bands of cellulose and glucomannan reveals that the two polymers move synchronously as a result of the applied strain. Furthermore, this suggests a strong interaction between the two polysaccharides inside the wood cell wall. Thus a strong coupling between the glucomannan aligned in parallel with the cellulose chains is anticipated. 3. Softwood Pulps When wood fibers are used for paper production, they are first exposed to a pulping process involving high temperatures and chemical reagents in order to remove the lignin. As mentioned earlier, during this process, other wood polymers, the cellulose and the hemicelluloses, are also affected. A˚kerholm and Salme´n [61] used 2-D FT-IR spectroscopy to investigate how different pulping processes affected the mechanical interaction between the cellulose and the hemicelluloses. In Figs. 29 and 30, dynamic inphase spectra at 0j and 90j polarization of three different chemical softwood pulps are plotted together with the corresponding spectra of holocellulose.
Figure 29 Dynamic in-phase FT-IR spectra at 0j polarization for holocellulose and three different chemical softwood pulps. The sheets are strained in the fiber direction.
178
Salme´n et al.
Figure 30 Dynamic in-phase FT-IR spectra at 90j polarization for holocellulose and three different chemical softwood pulps. The sheets are strained in the fiber direction.
Evidently, the dynamic FT-IR spectra are surprisingly similar in the fingerprint region for these pulps, and no large difference could be seen in the spectra between holocellulose pulp and the different chemical pulps of softwood. As for the holocellulose, only dynamic peaks from cellulose were found in the 0j polarization mode (Fig. 29). At 90j polarization, with the stretching parallel to the fiber direction (Fig. 30), dynamic peaks appeared both for cellulose and glucomannan for all samples. No dynamic signals from xylan were observed. This means that the interactions between glucomannan and cellulose that were established for the wood structure remained after the different pulping processes, while the xylan was
still unaffected by the applied strain in the fiber direction. This is probably also a consequence of the native construction of the wood cell wall. The cellulose-reinforced composite structure is not reorganized very much during the pulping processes. 4. Interaction Between Fibers As mentioned earlier in ‘‘Orientation Aspects,’’ the straining of a sheet of fibers perpendicular to the fiber direction results in loading conditions that are different from the loading of the sheet in the fiber direction. Because of the bending and shearing of the fibers in this loading mode,
Figure 31 Dynamic in-phase FT-IR spectra at 0j polarization of a kraft liner (thick line) and an acid sulfite pulp (thin line); fibers stretched perpendicular to fiber direction.
2D FT-IR Spectroscopy Applied to Cellulose and Paper
179
tions. In this case, there are also dynamic signals from the xylan for some of the pulps, showing that xylan is more important for the interfiber bonding than for the mechanical properties along the fiber axis. In Fig. 31, it can be seen that for a kraft liner pulp, a pulp containing 24% hemicellulose, a stronger dynamic response is obtained for the xylan (the band at 1730 cm1) than for the acid sulfite pulp of comparable chemical composition. This is probably due to the resorption of xylan on the fiber surfaces during kraft pulping in contrast to what occurs in sulfite pulping [122].
Figure 32 Dynamic in-phase FT-IR spectra of a birch kraft pulp (thin line) compared to a bleached softwood kraft pulp (thick line). The fibers are strained in the fiber direction and the upper spectra are recorded at 0j polarization, whereas the lower spectra are recorded at 90j polarization.
the straining of the structure reflects more the interactions in the transverse direction of the fibers and the interactions in the bonds between fibers. The dynamic spectra of sheets of pulp fibers are also different in these loading circumstances. When comparing spectra from 0j and 90j polarization modes, the orientational effect, which occurs for fibers loaded in the longitudinal direction, is not seen. In the first direction, there are dynamic signals from both cellulose and glucomannan in both the polarization direc-
5. Hardwood Pulps Hardwoods differ chemically from softwoods mainly in that they usually have a higher content of xylan in relation to the glucomannan. Other types of hemicellulose might also be present and the hardwood xylan contains acetyl groups but not arabinose substituents as softwood xylan. For a birch pulp, the content of glucomannan is very small, while much more xylan is present compared to softwood pulp fibers. Despite the large difference in chemical composition, the dynamic spectra of birch fibers [61] are very similar to those of softwood fibers (see Fig. 32). The main response in the dynamic spectra originates from the cellulose. No signals originating from xylan (the principle hemicellulose in birch) could be found in this case when the sheets were strained in the fiber direction. Again, this demonstrates the importance of the cellulose fibrils in determining the longitudinal fiber properties.
B. Lignin Interaction The mechanical properties of the cell wall lignin are especially important in determining the properties of mechanical pulp fibers. Even if almost all the lignin is removed
Figure 33 Static FT-IR spectrum for a mechanical pulp (thin line) plotted together with the corresponding spectrum for holocellulose (thick line).
180
from the chemically pulped and bleached fibers, a consideration of the viscoelastic properties of the cell wall lignin is still important for understanding the chemical pulping processes [118]. The vibrational spectrum of lignin differs from the spectrum of the wood polysaccharides in several wave number regions due to its aromatic structure [123,124]. This is evident from Fig. 33, which compares the static FT-IR spectrum of a holocellulose sheet with that of a lignin-rich thermomechanical pulp (TMP) sheet. Lignin, however, also has absorption bands in the areas where characteristic peaks of xylan and glucomannan are found. Applying 2-D FT-IR spectroscopy [60] to a lignincontaining pulp (Fig. 34) shows that in the 0j polarization mode, the spectra are very similar to those for lignin-free pulps (compare Fig. 34 with the spectra in Fig. 29). From the lignin characteristic vibrations, only a very weak negative signal at 1504 cm1 is seen in the dynamic inphase spectrum. This is not surprising though if the wood fiber is compared with a fiber-reinforced composite, here with cellulose as the reinforcement. In the fiber direction, the cellulose fibrils are the load-bearing elements. Since the dynamic spectra only show changes in spectral intensity, and the cellulose is the strained polymer, the dynamic spectra of the 0j polarization mode for all cellulose-reinforced materials ought to be very similar. Irrespective of whether the matrix material consists only of hemicelluloses or a mixture of hemicelluloses and lignin, it might be expected that there would only be signals originating from the cellulose fibrils when the matrix material is strained in the fiber direction. When detecting the signals at 90j polarization, the dynamic FT-IR spectra of a TMP sheet strained in the
Salme´n et al.
fiber direction contain different lignin-characteristic peaks (see Fig. 35). In the 90j polarization experiments, the spectra mainly show changes perpendicular to the straining direction. When most materials are strained, there will also be a dimensional change perpendicular to the straining direction (the Poison effect). For a fiber-reinforced composite, these transverse changes appear mainly in the matrix material. As seen in this polarization direction, the TMP spectra are considerably different from the dynamic spectra of lignin-free pulps (compare Figs. 23 and 35). For TMP, there is a large contribution from the viscous component (out of phase) of the dynamic spectrum with a number of peaks that refer to vibrations in the lignin macromolecule [60]. As for the polysaccharides, the lignin is well below its glass transition temperature under the measurement conditions and ought to be elastic in nature [118]. Secondary transitions in the lignin also exist [125], which ought to give an increased damping of the material. Such secondary transitions could be the reason for the high phase angles of the lignin vibrations. Mechanical spectra of spruce pulp fibers have actually been shown to have a slightly higher damping in fibers containing more than 10% lignin compared to lignin-free fibers [126]. In lignin, one secondary transition is attributed to the rotation of the methoxyl group [125], and most of the peaks marked in the out-ofphase spectrum in Fig. 35 are connected to the methoxyl group as different CH or CO vibrations. Why the aromatic vibration at about 1510 cm1 is affected and not the aromatic vibration at 1600 cm1 still has to be explained. The results above show that the lignin is contributing to the viscoelastic properties of the fiber as a matrix material capable of moving independently of the cellulose fibrils.
Figure 34 Dynamic FT-IR spectra of lignin-rich mechanical pulp (TMP) fiber sheets recorded at 0j polarization. The thin line represents the elastic part (in-phase), while the thick line represents the viscous part (out-of-phase) of the dynamic spectrum. The TMP sheets were strained in the fiber direction.
2D FT-IR Spectroscopy Applied to Cellulose and Paper
181
Figure 35 Dynamic FT-IR spectra of lignin-rich mechanical pulp (TMP) fiber sheets recorded at 90j polarization. The thin line represents the elastic part (in-phase), while the thick line represents the viscous part (out-of-phase) of the dynamic spectrum. The TMP sheets were strained in the fiber direction.
As there is a time-delayed response in the sinusoidally strained sheets of TMP fibers, the full advantage of the 2-D FT-IR technique can be explored. Compared to mechanical spectroscopy, dynamic 2-D FT-IR spectroscopy is much more sensitive in detecting specific time-delayed responses. With 2-D FT-IR spectroscopy, the time delay of each separate molecular vibration in the polymer mixture can be displayed as shown in Fig. 35. The different time delays of the different molecular vibrations enhance the resolution of the IR spectra (compare Figs. 33 and 35). Another advantage is the use of 2-D IR correlation spectra (Eqs. 7 and 8 of this chapter), which spread the spectral result over three dimensions which therefore facilitates interpretation. In Fig. 36, the synchronous 2-D IR correlation spectrum of a TMP fiber sheet (90j polarization) is shown for the 1550–1300 cm1 region. As described earlier, on the off-diagonal, there are cross-peaks between all synchronized vibrations. For instance, there are crosspeaks between the aromatic vibration at 1508 cm1 and the lignin-characteristic vibrations at 1430, 1373, 1339, and 1315 cm1. There are also cross-peaks between cellulose bands showing an elastic response such as the ones at 1462 and 1319 cm1. In Fig. 37, the corresponding asynchronous 2-D IR correlation spectrum is shown. This spectrum shows high correlation intensity (cross-peaks) for vibrations with different time-dependent behavior and consequently there are no peaks on the diagonal. In this case, there are, for instance, cross-peaks between the aromatic 1508-cm1 band and bands with an elastic response such as the cellulose bands at 1462, 1377, and 1319 cm1. It has recently been shown by polarized FT-IR measurements that lignin has an ordered structure within the
wood fiber wall [60]. The results show that the phenyl propane units are preferably oriented in the direction of the fiber axis. This ordered structure could be the reason for the different dynamic behavior in the 0j and 90j polarization measurements of the TMP.
C. Moisture Effects All of the wood polymers are hygroscopic and the absorbed moisture has a profound influence on the properties of wood fibers which are seen as dimensional changes, swell-
Figure 36 Synchronous 2-D FT-IR spectrum of a mechanical pulp fiber sheet measured in the 90j polarization direction.
182
Figure 37 Asynchronous 2-D FT-IR spectrum of a mechanical pulp fiber sheet measured in the 90j polarization direction.
ing, and effects on its mechanical properties. As water acts as a plasticizer, there is a drastic lowering of the softening temperature for the wood polymers under humid conditions [125]. This effect is of particular relevance when selecting a temperature for the mechanical pulping process or by introducing moisture and/or heat during calendering. Effects of moisture on the elastic modulus have been determined both for paper [127] and for extracted hemicelluloses [128] and lignin [129]. Close to their softening points, polymers clearly exhibit a viscoelastic behavior which is why mechanical spectroscopy provides a good tool for characterizing the influence of different components on the mechanical properties [125]. This also applies for wood fibers [130]. Since 2-D FT-IR spectroscopy provides the elastic and viscous component of each molecular vibration, this method provides a means of revealing the behavior of the components, and even the molecular groups, in their contribution to the softening of a composite material. In general, IR studies under moist conditions can be problematic because of the many broad absorption bands associated with water and the changes in these as moisture levels around the sample are changed. To overcome this, the use of a mechanism to precisely control the environment around the sample is necessary. By placing the polymer stretcher in a heated moisture chamber (Manning Applied Technologies Inc., Troy, ID, U.S.A.) connected to an accurate humidity generator, it is possible to perform 2-D FT-IR experiments under humid conditions. As far as wood polymers are concerned, the use of temperatures up to 40jC and high humidities in measurements would result in viscous contributions mainly from the hemicelluloses, which ought to be softened in this region [128,131]. Fig. 38 shows the dynamic 2-D FT-IR spectra of a spruce holocellulose measured at room temperature and 0% relative humidity (RH) compared to similar measurements at 40jC and 90%RH. A small increase of
Salme´n et al.
the viscous component can be seen for the spectra measured under humid conditions, especially in the low-wave number region. This indicates that the polymers are closer to a transition point and more time-dependent responses are shown. The spectra illustrated were recorded at 90j polarization and are more indicative of the response of the matrix material; this increased viscoelasticity must therefore be attributed to the hemicelluloses within the fiber material. The dynamic spectra at 0j polarization which reflect the cellulose straining (‘‘Hemicellulose interaction’’) show no increase in the viscous component for the holocellulose measured at 90%RH and 40jC. In the 90j polarization mode, the high response of the out-ofphase spectrum can mainly be seen for the characteristic peaks of glucomannan at 810 and 870 cm1, in the area between 1040 and 1080 cm1, and also, to some extent, at some of the higher wave numbers. In the 1040- and 1080cm1 area, characteristic peaks of galactose, side groups of glucomannan, have been reported [119,132]. There are, however, several strong cellulose bands in this region also, consisting of highly coupled motions dominated by CC and CO stretching with small contribution from HCC, HCO, and skeletal atom bending [98]. From the PLS analysis of alkali extracted holocelluloses (Fig. 21) described earlier in this chapter, it can be seen that both xylan and glucomannan contribute strongly to the absorption in this area. Although a softening of the xylan and the glucomannan is probable under the high humidity conditions used, there are no viscous signals from the
Figure 38 Dynamic FT-IR spectra of spruce holocellulose recorded at 90j polarization. The thin lines represent in-phase spectra and the thick lines represent out-of-phase spectra. The upper spectra are recorded at 0%RH and room temperature, whereas the lower spectra are recorded at 90%RH and 40jC.
2D FT-IR Spectroscopy Applied to Cellulose and Paper
characteristic xylan vibrations at 1600 and 1730 cm1. These signals originate from side groups of the polymer chain and may not be affected to the same extent as the main chain when the fibers are subjected to loading. The region between 1150 and 1270 cm1 contains both skeletal stretching vibrations as well as methine bending and is sensitive to the orientation of the glycosidic linkage [98]. This region is also affected by changes in the environment, but here it is mainly the in-phase spectrum that shows the changes. The peak at 1169 cm1 in the in-phase spectrum recorded under dry conditions is split into one peak at 1150 cm1 and one peak at 1184 cm1 in the same spectrum recorded under humid conditions. The induced softening of the hemicelluloses might result in movements of polymer segments and thereby result in spectral changes in this area. In Fig. 39, the dynamic spectra for the different environments, 0%RH and 90%RH, are also compared for a chemithermomechanical pulp (CTMP). The 0%RH spectrum indicates a greater degree of viscoelasticity than the corresponding spectrum of the holocellulose. The degree of viscoelasticity may be quantified from the phase angle of the spectra, where an elastic material has a phase angle of 0j and a viscous material has a phase angle of 90j. From the dynamic IR spectra, a mean phase angle can be calculated for a selected wave number range using the absolute values of the in-phase and out-of-phase spectra. For the holocellulose spectra shown in Fig. 38, there is an
183
increase in phase angle from 15j to 37j going from 0%RH, 25jC to 90%RH, 40jC. The corresponding values for the CTMP spectra in Fig. 39 are from 28j to 35j. The CTMP obviously has a higher viscous response even in the dry state as was discussed earlier in this section in which measurements on TMP were discussed. There is, however, a lower increase in viscosity as a result of the changed environment for the lignin-rich pulp compared to the holocellulose. There is also a considerable difference in the plasticizing effect that water has on the lignin component as compared to the hemicelluloses. Because of its cross-linked structure, the glass transition temperature (Tg) of lignin can only be reduced to about 75jC through absorption of moisture [133], while the Tg of the hemicelluloses may be reduced to room temperature [118]. In the in-phase spectrum of the CTMP recorded under moist conditions (Fig. 39), a broad signal with its maximum at 1630 cm1 can be seen, which is absent from the spectrum measured under dry conditions. This signal probably originates from a deformation vibration of molecularly adsorbed water [134]. It has been shown that the moisture content of paper increases under mechanical load under humid conditions, both by measurements using an analytical balance [135] and by NIR measurements [136]. The appearance of this peak in the in-phase spectrum also shows the instantaneous change of adsorbed water as a result of the small dynamic strain applied. The fact that this peak is not as apparent in the spectrum of holocellulose under humid conditions (Fig. 38) could be a consequence of the greater number of charged groups in the CTMP capable of holding a higher volume of water. This effect has also been shown for a birch pulp with a large number of charged groups [137].
V. FUTURE DEVELOPMENTS
Figure 39 Dynamic FT-IR spectra of a spruce chemithermomechanical pulp recorded at 90j polarization. The thin lines represent in-phase spectra and the thick lines represent out-of-phase spectra. The upper spectra are recorded at 0%RH and room temperature, whereas the lower spectra are recorded at 90%RH and 40jC.
From the studies described, it is clear that 2-D FT-IR represents a powerful tool for increasing our knowledge of cellulose structure and the dynamic behavior of isolated cellulose, as well as of the wood polymers in fibers. One of the key points is that it provides a possibility for studying the interactions within biopolymers. 2-D FT-IR is a tool for elucidating interactions in biological assembles at the molecular level. There is still a lack of systematic fundamental work on, for instance, different cellulose polymorphs as well as different types of hemicelluloses that could provide a more exact assignment of different dynamic IR bands. One of the main problems associated with transmittance 2-D FT-IR is the prerequisite for thin sheets in the equipment. A development toward a reflectance application could hence be of great benefit, although mostly surface-type behavior would be observed.
REFERENCES 1.
Jones, E.J. The infrared spectrum of spruce native lignin. J. Am. Chem. Soc. 1948, 70, 1984.
Salme´n et al.
184 2. 3. 4.
5. 6. 7. 8.
9. 10. 11.
12.
13. 14. 15.
16. 17. 18. 19. 20.
21.
22.
Lange, P.W. Ultraviolettabsorption av fast lignin. Sven. Papp.tidn. 1945, 48, 241. Freudenberg, K.; Siebert, W.; Heimberger, W.; Kraft, R. Ultrarotspektren von Lignin und lignina¨hnlichen Stoffen. Ber. Dtsche. Chem. Ges. 1950, 83, 533. Tschalmer, H.; Kratzl, K.; Leutner, R.; Steininger, A.; Kisser, J. Die Ultrarotspektren mikroskopischer Holzschnitte und einiger Modellsubstanzen. Mikrosk./Zent.bl. Mikrosk. Forsch. Method. 1953, 8, 238. Tsuboi, M. Infrared spectrum and crystal structure of cellulose. J. Polym. Sci. 1957, 25, 159. Liang, C.Y.; March