Landolt-Börnstein Numerical Data and Functional Relationships in Science and Technology New Series / Editor in Chief: W. Martienssen
Group IV: Physical Chemistry Volume 11
Ternary Alloy Systems Phase Diagrams, Crystallographic and Thermodynamic Data critically evaluated by MSIT® Subvolume E Refractory Metal Systems Part 1 Selected Systems from Al-B-C to B-Hf-W Editors G. Effenberg and S. Ilyenko
Authors Materials Science and International Team, MSIT®
ISSN
1615-2018 (Physical Chemistry)
ISBN
978-3-540-88052-3 Springer Berlin Heidelberg New York
Library of Congress Cataloging in Publication Data Zahlenwerte und Funktionen aus Naturwissenschaften und Technik, Neue Serie Editor in Chief: W. Martienssen Vol. IV/11E1: Editors: G. Effenberg, S. Ilyenko At head of title: Landolt-Börnstein. Added t.p.: Numerical data and functional relationships in science and technology. Tables chiefly in English. Intended to supersede the Physikalisch-chemische Tabellen by H. Landolt and R. Börnstein of which the 6th ed. began publication in 1950 under title: Zahlenwerte und Funktionen aus Physik, Chemie, Astronomie, Geophysik und Technik. Vols. published after v. 1 of group I have imprint: Berlin, New York, Springer-Verlag Includes bibliographies. 1. Physics--Tables. 2. Chemistry--Tables. 3. Engineering--Tables. I. Börnstein, R. (Richard), 1852-1913. II. Landolt, H. (Hans), 1831-1910. III. Physikalisch-chemische Tabellen. IV. Title: Numerical data and functional relationships in science and technology. QC61.23 502'.12 62-53136 This work is subject to copyright. All rights are reserved, whether the whole or part of the material is concerned, specifically the rights of translation, reprinting, reuse of illustrations, recitation, broadcasting, reproduction on microfilm or in other ways, and storage in data banks. Duplication of this publication or parts thereof is permitted only under the provisions of the German Copyright Law of September 9, 1965, in its current version, and permission for use must always be obtained from Springer-Verlag. Violations are liable for prosecution act under German Copyright Law. Springer is a part of Springer Science+Business Media springeronline.com © Springer-Verlag Berlin Heidelberg 2009 Printed in Germany The use of general descriptive names, registered names, trademarks, etc. in this publication does not imply, even in the absence of a specific statement, that such names are exempt from the relevant protective laws and regulations and therefore free for general use. Product Liability: The data and other information in this handbook have been carefully extracted and evaluated by experts from the original literature. Furthermore, they have been checked for correctness by authors and the editorial staff before printing. Nevertheless, the publisher can give no guarantee for the correctness of the data and information provided. In any individual case of application, the respective user must check the correctness by consulting other relevant sources of information. Cover layout: Erich Kirchner, Heidelberg Typesetting: Materials Science International Services GmbH, Stuttgart Printing and Binding: AZ Druck, Kempten/Allgäu
SPIN: 1091 6131
63/3020 - 5 4 3 2 1 0 – Printed on acid-free paper
Editors: Associate Editor:
Günter Effenberg Svitlana Ilyenko Oleksandr Dovbenko
MSI, Materials Science International Services GmbH Postfach 800749, D-70507, Stuttgart, Germany http://www.matport.com
Authors: Materials Science International Team, MSIT® The present series of books results from collaborative evaluation programs performed by MSI and authored by MSIT®. In this program data and knowledge are contributed by many individuals and accumulated over almost twenty years, now. The content of this volume is a subset of the ongoing MSIT® Evaluation Programs. Authors of this volume are: Zoya Alekseeva, Moscow, Russia
Jozefien De Keyzer, Heverlee, Belgium
Christian Bätzner, Stuttgart, Germany
Natalia Kol’chugina, Moscow, Russia
Natalia Bochvar, Moscow, Russia
Kostyantyn Korniyenko, Kyiv, Ukraine
Anatoliy Bondar, Kyiv, Ukraine
Artem Kozlov, Clausthal-Zellerfeld, Germany
Jörg Beuers, Hanau, Germany Gabriele Cacciamani, Genova, Italy Andriy Grytsiv, Vienna, Austria Lesley Cornish, Randburg, South Africa
Vasyl Kublii, Kyiv, Ukraine Viktor Kuznetsov, Moscow, Russia Nathalie Lebrun, Lille, France Hans Leo Lukas, Stuttgart, Germany Annelies Malfliet, Heverlee, Belgium
Damian M. Cupid, Freiberg, Germany Dmytro Pavlyuchkov, Jülich, Germany Tatiana Dobatkina, Moscow, Russia Oleksandr Dovbenko, Stuttgart, Germany Guenter Effenberg, Stuttgart, Germany Ol’ga Fabrichnaya, Freiberg, Germany Sergio Gama, Campinas, Brazil
Pierre Perrot, Lille, France Qingsheng Ran, Stuttgart, Germany Peter Rogl, Vienna, Austria Lazar Rokhlin, Moscow, Russia Eberhard E. Schmid, Frankfurt, Germany
Joachim Gröbner, Clausthal-Zellerfeld, Germany An Serbruyns, Heverlee, Belgium Mireille Harmelin, Paris, France
Elena Semenova, Kyiv, Ukraine
Frederick H. Hayes, Manchester, UK
Jean-Claude Tedenac, Montpellier, France
Michael Hoch, Cincinnati, USA
Vasyl Tomashik, Kyiv, Ukraine
Svitlana Ilyenko, Stuttgart, Germany
Mikhail Turchanin, Kramatorsk, Ukraine
Volodymyr Ivanchenko, Kyiv, Ukraine
Tamara Velikanova, Kyiv, Ukraine
Institutions The content of this volume is produced by MSI, Materials Science International Services GmbH and the international team of materials scientists, MSIT®. Contributions to this volume have been made from the following institutions:
The Baikov Institute of Metallurgy, Academy of Sciences, Moscow, Russia Degussa AG, Hanau, Germany Donbass State Mechanical Engineering Academy, Kramatorsk, Ukraine Forschungszentrum Jülich, Institut für Festkörperforschung (IFF), Institut Mikrostrukturforschung, Jülich, Germany I.M. Frantsevich Institute for Problems of Materials Science, National Academy of Sciences, Kyiv, Ukraine Institute for Semiconductor Physics, National Academy of Sciences, Kyiv, Ukraine Katholieke Universiteit Leuven, Department Metaalkunde en Toegepaste Materiaalkunde, Heverlee, Belgium G.V. Kurdyumov Institute for Metal Physics, National Academy of Sciences, Kyiv, Ukraine Materials Science International Services GmbH, Stuttgart, Germany Max-Planck-Institut für Metallforschung, Institut für Werkstoffwissenschaft, Pulvermetallurgisches Laboratorium, Stuttgart, Germany Moscow State University, Department of General Chemistry, Moscow, Russia
School of Chemical and Metallurgical Engineering, The University of the Witwatersrand, DST/NRF Centre of Excellence for Strong Material, South Afrika Technische Universität Bergakademie Freiberg, Institut für Werkstoffwissenschaft, Freiberg, Germany Technische Universität Clausthal, Metallurgisches Zentrum, Clausthal-Zellerfeld, Germany Universidade Estadual de Campinas, Instituto de Fisica “Gleb Wataghin”, DFESCM, Campinas, Brazil Universita di Genova, Dipartimento di Chimica, Genova, Italy Universität Wien, Institut für Physikalische Chemie, Wien, Austria Universite de Lille I, Laboratoire de Métallurgie Physique, Villeneuve d’ASCQ, France Universite de Montpellier II, Laboratorie de Physico-chimie de la Materiere Montpellier, France University of Cincinnati, Department of Materials Science and Engineering, Cincinnati, USA
Preface The sub-series Ternary Alloy Systems of the Landolt-Börnstein New Series provides reliable and comprehensive descriptions of the materials constitution, based on critical intellectual evaluations of all data available at the time and it critically weights the different findings, also with respect to their compatibility with today’s edge binary phase diagrams. Selected are ternary systems of importance to alloy development and systems which gained in the recent years otherwise scientific interest. In one ternary materials system, however, one may find alloys for various applications, depending on the chosen composition. Reliable phase diagrams provide scientists and engineers with basic information of eminent importance for fundamental research and for the development and optimization of materials. So collections of such diagrams are extremely useful, if the data on which they are based have been subjected to critical evaluation, like in these volumes. Critical evaluation means: there where contradictory information is published data and conclusions are being analyzed, broken down to the firm facts and re-interpreted in the light of all present knowledge. Depending on the information available this can be a very difficult task to achieve. Critical evaluations establish descriptions of reliably known phase configurations and related data. The evaluations are performed by MSIT®, Materials Science International Team, a group of scientists working together since 1984. Within this team skilled expertise is available for a broad range of methods, materials and applications. This joint competence is employed in the critical evaluation of the often conflicting literature data. Particularly helpful in this are targeted thermodynamic and atomistic calculations for individual equilibria, driving forces or complete phase diagram sections. Conclusions on phase equilibria may be drawn from direct observations e.g. by microscope, from monitoring caloric or thermal effects or measuring properties such as electric resistivity, electro-magnetic or mechanical properties. Other examples of useful methods in materials chemistry are massspectrometry, thermo-gravimetry, measurement of electro-motive forces, X-ray and microprobe analyses. In each published case the applicability of the chosen method has to be validated, the way of actually performing the experiment or computer modeling has to be validated as well and the interpretation of the results with regard to the material’s chemistry has to be verified. Therefore insight in materials constitution and phase reactions is gained from many distinctly different types of experiments, calculation and observations. Intellectual evaluations which interpret all data simultaneously reveal the chemistry of the materials system best. An additional degree of complexity is introduced by the material itself, as the state of the material under test depends heavily on its history, in particular on the way of homogenization, thermal and mechanical treatments. All this is taken into account in an MSIT® expert evaluation. To include binary data in the ternary evaluation is mandatory. Each of the three-dimensional ternary phase diagrams has edge binary systems as boundary planes; their data have to match the ternary data smoothly. At the same time each of the edge binary systems A-B is a boundary plane for many other ternary A-B-X systems. Therefore combining systematically binary and ternary evaluations increases confidence and reliability in both ternary and binary phase diagrams. This has started systematically for the first time here, by the MSIT® Evaluation Programs applied to the Landolt-Börnstein New Series. The degree of success, however, depends on both the nature of materials and scientists! The multitude of correlated or inter-dependant data requires special care. Within MSIT® an evaluation routine has been established that proceeds knowledge driven and applies both, human based expertise and electronically formatted data and software tools. MSIT® internal discussions take place in almost all evaluation works and on many different specific questions the competence of a team is added to the work of individual authors. In some cases the authors of earlier published work contributed to the knowledge
base by making their original data records available for re-interpretation. All evaluation reports published here have undergone a thorough review process in which the reviewers had access to all the original data. In publishing we have adopted a standard format that presents the reader with the data for each ternary system in a concise and consistent manner, as applied in the “MSIT® Workplace Phase Diagrams Online”. The standard format and special features of the Landolt-Börnstein compendium are explained in the Introduction to the volume. In spite of the skill and labor that have been put into this volume, it will not be faultless. All criticisms and suggestions that can help us to improve our work are very welcome. Please contact us via
[email protected]. We hope that this volume will prove to be as useful for the materials scientist and engineer as the other volumes of Landolt-Börnstein New Series and the previous works of MSIT® have been. We hope that the Landolt Börnstein Sub-series, Ternary Alloy Systems will be well received by our colleagues in research and industry. On behalf of the participating authors we want to thank all those who contributed their comments and insight during the evaluation process. In particular we thank the reviewers - Pierre Perrot, Tamara Velikanova, Hans Leo Lukas, Marina Bulanova, Mikhail Turchanin, Nataliya Bochvar, Olga Fabrichnaya and Viktor Kuznetsov. We all gratefully acknowledge the dedicated scientific desk editing by Oleksandra Berezhnytska, Mariya Saltykova and Oleksandr Rogovtsov.
Günter Effenberg, Svitlana Ilyenko and Oleksandr Dovbenko
Stuttgart, June 2008
Contents IV/11E1 Ternary Alloy Systems Phase Diagrams, Crystallographic and Thermodynamic Data Subvolume E Refractory Metal Systems Part 1 Selected Systems from Al-B-C to B-Hf-W Introduction Data Covered..........................................................................................................................................XI General ...................................................................................................................................................XI Structure of a System Report .................................................................................................................XI Introduction....................................................................................................................................XI Binary Systems ..............................................................................................................................XI Solid Phases ................................................................................................................................. XII Quasibinary Systems...................................................................................................................XIII Invariant Equilibria .....................................................................................................................XIII Liquidus, Solidus, Solvus Surfaces ............................................................................................XIII Isothermal Sections.....................................................................................................................XIII Temperature – Composition Sections ........................................................................................XIII Thermodynamics.........................................................................................................................XIII Notes on Materials Properties and Applications........................................................................XIII Miscellaneous .............................................................................................................................XIII References ...................................................................................................................................XVI General References ........................................................................................................................... XVII
Ternary Systems Al – B – C (Aluminium – Boron – Carbon) ...........................................................................................1 Al – B – Mo (Aluminium – Boron – Molybdenum) ............................................................................24 Al – B – Si (Aluminium – Boron – Silicon) .........................................................................................33 Al – C – Ti (Aluminium – Carbon – Titanium)....................................................................................41 Al – Cr – Ti (Aluminium – Chromium – Titanium).............................................................................72 Al – Fe – Nb (Aluminium – Iron – Niobium).....................................................................................109 Al – Mo – Ni (Aluminium – Molybdenum – Nickel) ........................................................................123 Al – Mo – U (Aluminium – Molybdenum – Uranium) ......................................................................144 Al – Nb – Ni (Aluminium – Niobium – Nickel).................................................................................164 Al – Nb – Si (Aluminium – Niobium – Silicon).................................................................................193 Al – Ni – V (Aluminium – Nickel – Vanadium) ................................................................................209 Al – O – Zr (Aluminium – Oxygen – Zirconium) ..............................................................................225 Al – Ta – Ti (Aluminium – Tantalum – Titanium).............................................................................242 B – C – Cr (Boron – Carbon – Chromium) ........................................................................................261 B – C – Hf (Boron – Carbon – Hafnium) ...........................................................................................282 B – C – Mo (Boron – Carbon – Molybdenum)...................................................................................306
B – C – N (Boron – Carbon – Nitrogen).............................................................................................323 B – C – Nb (Boron – Carbon – Niobium)...........................................................................................347 B – C – Si (Boron – Carbon – Silicon) ...............................................................................................367 B – C – Ta (Boron – Carbon – Tantalum) ..........................................................................................395 B – C – V (Boron – Carbon – Vanadium) ..........................................................................................408 B – C – W (Boron – Carbon – Tungsten) ...........................................................................................427 B – C – Zr (Boron – Carbon – Zirconium) .........................................................................................450 B – Cr – Mn (Boron – Chromium – Manganese) ...............................................................................476 B – Cr – Ti (Boron – Chromium – Titanium).....................................................................................485 B – Cr – Zr (Boron – Chromium – Zirconium) ..................................................................................494 B – Fe – Mo (Boron – Iron – Molybdenum) ......................................................................................500 B – Hf – Mo (Boron – Hafnium – Molybdenum) ..............................................................................514 B – Hf – W (Boron – Hafnium – Tungsten) .......................................................................................523
Introduction
1
Introduction Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data
Data Covered The series focuses on light metal ternary systems and includes phase equilibria of importance for alloy development, processing or application, reporting on selected ternary systems of importance to industrial light alloy development and systems which gained otherwise scientific interest in the recent years.
General The series provides consistent phase diagram descriptions for individual ternary systems. The representation of the equilibria of ternary systems as a function of temperature results in spacial diagrams whose sections and projections are generally published in the literature. Phase equilibria are described in terms of liquidus, solidus and solvus projections, isothermal and pseudobinary sections; data on invariant equilibria are generally given in the form of tables. The world literature is thoroughly and systematically searched back to the year 1900. Then, the published data are critically evaluated by experts in materials science and reviewed. Conflicting information is commented upon and errors and inconsistencies removed wherever possible. It considers those, and only those data, which are firmly established, comments on questionable findings and justifies re-interpretations made by the authors of the evaluation reports. In general, the approach used to discuss the phase relationships is to consider changes in state and phase reactions which occur with decreasing temperature. This has influenced the terminology employed and is reflected in the tables and the reaction schemes presented. The system reports present concise descriptions and hence do not repeat in the text facts which can clearly be read from the diagrams. For most purposes the use of the compendium is expected to be self-sufficient. However, a detailed bibliography of all cited references is given to enable original sources of information to be studied if required.
Structure of a System Report The constitutional description of an alloy system consists of text and a table/diagram section which are separated by the bibliography referring to the original literature (see Fig. 1). The tables and diagrams carry the essential constitutional information and are commented on in the text if necessary. Where published data allow, the following sections are provided in each report: Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
1
2
1
Introduction
. Fig. 1 Structure of a system report
Introduction The opening text reviews briefly the status of knowledge published on the system and outlines the experimental methods that have been applied. Furthermore, attention may be drawn to questions which are still open or to cases where conclusions from the evaluation work modified the published phase diagram.
Binary Systems Where binary systems are accepted from standard compilations reference is made to these compilations. In other cases the accepted binary phase diagrams are reproduced for the convenience of the reader. The selection of the binary systems used as a basis for the evaluation of the ternary system was at the discretion of the assessor. DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Introduction
1
Solid Phases The tabular listing of solid phases incorporates knowledge of the phases which is necessary or helpful for understanding the text and diagrams. Throughout a system report a unique phase name and abbreviation is allocated to each phase. Phases with the same formulae but different space lattices (e.g. allotropic transformation) are distinguished by:
– small letters (h), high temperature modification (h2 > h1) (r), room temperature modification (1), low temperature modification (l1 > l2) – Greek letters, e.g., ε, ε´ – Roman numerals, e.g., (I) and (II) for different pressure modifications. In the table “Solid Phases” ternary phases are denoted by * and different phases are separated by horizontal lines.
Quasibinary Systems Quasibinary (pseudobinary) sections describe equilibria and can be read in the same way as binary diagrams. The notation used in quasibinary systems is the same as that of vertical sections, which are reported under “Temperature – Composition Sections”.
Invariant Equilibria The invariant equilibria of a system are listed in the table “Invariant Equilibria” and, where possible, are described by a constitutional “Reaction Scheme” (Fig. 2). The sequential numbering of invariant equilibria increases with decreasing temperature, one numbering for all binaries together and one for the ternary system. Equilibria notations are used to indicate the reactions by which phases will be
– decomposed (e- and E-type reactions) – formed (p- and P-type reactions) – transformed (U-type reactions) ¨ bergangsreaktion) is used in order to reserve the For transition reactions the letter U (U letter T to denote temperature. The letters d and D indicate degenerate equilibria which do not allow a distinction according to the above classes.
Liquidus, Solidus, Solvus Surfaces The phase equilibria are commonly shown in triangular coordinates which allow a reading of the concentration of the constituents in at.%. In some cases mass% scaling is used for better data readability (see Figs. 3 and 4). Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
3
1
Introduction
. Fig. 2 Typical reaction scheme
4
DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Introduction
1
In the polythermal projection of the liquidus surface, monovariant liquidus grooves separate phase regions of primary crystallization and, where available, isothermal lines contour the liquidus surface (see Fig. 3).
Isothermal Sections Phase equilibria at constant temperatures are plotted in the form of isothermal sections (see Fig. 4).
Temperature – Composition Sections Non-quasibinary T-x sections (or vertical sections, isopleths, polythermal sections) show the phase fields where generally the tie lines are not in the same plane as the section. The notation employed for the latter (see Fig. 5) is the same as that used for binary and pseudobinary phase diagrams.
. Fig. 3 Hypothetical liquidus surface showing notation employed
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
5
6
1
Introduction
. Fig. 4 Hypothetical isothermal section showing notation employed
Thermodynamics Experimental ternary data are reported in some system reports and reference to thermodynamic modelling is made.
Notes on Materials Properties and Applications Noteworthy physical and chemical materials properties and application areas are briefly reported if they were given in the original constitutional and phase diagram literature.
Miscellaneous In this section noteworthy features are reported which are not described in preceding paragraphs. These include graphical data not covered by the general report format, such as lattice spacing – composition data, p-T-x diagrams, etc. DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Introduction
1
. Fig. 5 Hypothetical vertical section showing notation employed
References The publications which form the bases of the assessments are listed in the following manner: [1974Hay] Hayashi, M., Azakami, T., Kamed, M., “Effects of Third Elements on the Activity of Lead in Liquid Copper Base Alloys” (in Japanese), Nippon Kogyo Kaishi, 90, 51–56 (1974) (Experimental, Thermodyn., 16) This paper, for example, whose title is given in English, is actually written in Japanese. It was published in 1974 on pages 51- 56, volume 90 of Nippon Kogyo Kaishi, the Journal of the Mining and Metallurgical Institute of Japan. It reports on experimental work that leads to thermodynamic data and it refers to 16 cross-references. Additional conventions used in citing are: # to indicate the source of accepted phase diagrams * to indicate key papers that significantly contributed to the understanding of the system. Standard reference works given in the list “General References” are cited using their abbreviations and are not included in the reference list of each individual system.
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
7
8
1
Introduction
General References [C.A.] [Curr.Cont.] [E] [G] [H] [L-B]
[Mas] [Mas2] [P] [S] [V-C] [V-C2]
Chemical Abstracts - pathways to published research in the world’s journal and patent literature http://www.cas.org/ Current Contents - bibliographic multidisciplinary current awareness Web resource - http://www.isinet. com/products/cap/ccc/ Elliott, R.P., Constitution of Binary Alloys, First Supplement, McGraw-Hill, New York (1965) Gmelin Handbook of Inorganic Chemistry, 8th ed., Springer-Verlag, Berlin Hansen, M. and Anderko, K., Constitution of Binary Alloys, McGraw-Hill, New York (1958) Landolt-Boernstein, Numerical Data and Functional Relationships in Science and Technology (New Series). Group 3 (Crystal and Solid State Physics), Vol. 6, Eckerlin, P., Kandler, H. and Stegherr, A., Structure Data of Elements and Intermetallic Phases (1971); Vol. 7, Pies, W. and Weiss, A., Crystal Structure of Inorganic Compounds, Part c, Key Elements: N, P, As, Sb, Bi, C (1979); Group 4: Macroscopic and Technical Properties of Matter, Vol. 5, Predel, B., Phase Equilibria, Crystallographic and Thermodynamic Data of Binary Alloys, Subvol. a: Ac-Au … Au-Zr (1991); Springer-Verlag, Berlin. Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, ASM, Metals Park, Ohio (1986) Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Pearson, W.B., A Handbook of Lattice Spacings and Structures of Metals and Alloys, Pergamon Press, New York, Vol. 1 (1958), Vol. 2 (1967) Shunk, F.A., Constitution of Binary Alloys, Second Supplement, McGraw-Hill, New York (1969) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, ASM, Metals Park, Ohio (1985) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
DOI: 10.1007/978-3-540-88053-0_1 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Index of Alloy Systems
2
Index of Alloy Systems Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data
Index of Ternary Refractory Metal Alloy Systems Al-B-C to B-Hf-W
Al-B-C (Aluminium - Boron - Carbon) Al-B-Mo (Aluminium - Boron - Molybdenum) Al-B-Si (Aluminium - Boron - Silicon) Al-C-Ti (Aluminium - Carbon - Titanium) Al-Cr-Ti (Aluminium - Chromium - Titanium) Al-Fe-Nb (Aluminium - Iron - Niobium) Al-Mo-Ni (Aluminium - Molybdenum - Nickel) Al-Mo-U (Aluminium - Molybdenum - Uranium) Al-Nb-Ni (Aluminium - Niobium - Nickel) Al-Nb-Si (Aluminium - Niobium - Silicon) Al-Ni-V (Aluminium - Nickel - Vanadium) Al-O-Zr (Aluminium - Oxygen - Zirconium) Al-Ta-Ti (Aluminium - Tantalum - Titanium) B-C-Cr (Boron - Carbon - Chromium) B-C-Hf (Boron - Carbon - Hafnium) B-C-Mo (Boron - Carbon - Molybdenum) B-C-N (Boron - Carbon - Nitrogen) B-C-Nb (Boron - Carbon - Niobium) B-C-Si (Boron - Carbon - Silicon) B-C-Ta (Boron - Carbon - Tantalum) B-C-V (Boron - Carbon - Vanadium) B-C-W (Boron - Carbon - Tungsten) B-C-Zr (Boron - Carbon - Zirconium) B-Cr-Mn (Boron - Chromium - Manganese) B-Cr-Ti (Boron - Chromium - Titanium) B-Cr-Zr (Boron - Chromium - Zirconium) B-Fe-Mo (Boron - Iron - Molybdenum) B-Hf-Mo (Boron - Hafnium - Molybdenum) B-Hf-W (Boron - Hafnium - Tungsten)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_2 ß Springer 2009
1
Al–B–C
3
Aluminium – Boron – Carbon Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Andriy Grytsiv, Peter Rogl
Introduction Due to the presence of carbon contaminant in aluminium borides the data on the constitution of the Al-B-C ternary system and those of the binary Al-B system have to be reviewed carefully, which was done by [1994Dus] to strictly differentiate between true aluminium borides and aluminium boron carbides. High hardness in combination with high neutron absorption, high wear resistance and impact resistance have triggered an early interest in high-strength and low-weight Al-B4C composite materials or cermets, either in bulk form with a metal binder or by reinforcing an Al-base matrix with boron carbide particles or with boron carbide-coated fibres. Understanding the phase equilibria proved of major importance in the processing of Al-B4C composites particular in finding processing criteria at temperatures high enough to promote wetting and low enough to control reactions and design microstructures. Despite much effort was spent on the synthesis and crystallographic characterization of the various ternary aluminum boron carbide compounds [1964Mat, 1965Eco, 1965Mat, 1966Gie, 1966Lip, 1969Per, 1969Wil, 1970Nei, 1977Mat, 1987Sar, 1980Ino, 1990Oka, 1992Via, 1994Kud, 1995Osc, 1996Hil1, 1996Hil2, 1997Mey], information on the equilibrium phase relations in the Al-B-C ternary system is scarce [1993Bau, 1997Via, 1998Rog]. These informations comprise early calculations of the phase equilibria disregarding the boron-rich compounds or rather assuming the phases, AlB40C4 and Al2.1B51C8, to be part of the solid solution range of “B4C” [1982Doe, 1993Kau]. Some confusion in the early experimental work on aluminum borides arose from the fact that due to contamination either from high carbon level boron starting material or from the use of graphite crucibles and substrates aluminum boron carbides were produced rather than binary aluminum borides. This is particularly true for “AlB10” [1963Wil] - shown to be “AlB24C4” or more precisely Al2.1B51C8 [1964Mat, 1967Wil, 1969Wil, 1969Per, 1990Oka] - and βAlB12 [1960Koh], later shown to be Al3B48C2 [1965Mat]. According to structural and DTA investigations [1996Hil1], Al3B48C2 exists in a tetragonal high temperature modification, which on cooling below 650˚C transforms into a bodycentered orthorhombic low temperature phase with a unique structure type. The mixture of two orthorhombic phases with coherent boundary and commensurable lattice parameters (modifications A and B), as claimed by [1965Mat, 1986Pes], thus simply explains by multiple twinning on cooling [1996Hil1]. An experimental study of the isothermal section at 1400˚C by [1993Bau] confirmed the existence of four ternary compounds Al2.1B51C8 [1964Mat, 1967Wil, 1969Wil, 1969Per], AlB40C4 [1966Gie, 1966Lip, 1970Nei], Al3B48C2 [1996Hil1] and Al3BC3 [1996Hil2]. The latter compound was first mentioned as “Al4B1–3C4” [1964Mat] and later labelled as “Al8B4C7” [1980Ino] from a cursory investigation of its crystal symmetry with X-ray single crystal Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
1
2
3
Al–B–C
photographs, although no details of the crystal structure were derived. The relation to a wurtzite structure was discussed [1995Osc]. A structure determination is due to [1996Hil2]. A fifth compound, Al3BC [1992Via, 1993Gon, 1997Mey, 2002Zhe], (earlier “Al4BC” [1987Sar, 1989Hal, 1990Pyz]) was reported to exist below 1000˚C [1992Via], however, was shown in the isothermal section at 1000˚C [1997Via]. From a detailed analysis (XPD, LOM, SEM, EPMA) of the Al-rich corner [1997Via] on about 30 specimens prepared from cold pressed and sintered powder compacts in the temperature region from 627 to 1000˚C, an isothermal section at 1000˚C and a tentative liquidus projection was derived assisted by a series of isothermal diffusion experiments by heating together in an alumina boat an Al-B rod and an Al-C rod. Phase equilibria at 900˚C in the Al-C rich part of the ternary Al-B-C system were established [2002Zhe] from XPD of about 45 ternary and binary alloys. Equilibrium conditions were not reached for boron-rich samples. An attempt to obtain equilibrated samples from mixtures B4C+AlB2, B4C+Al and B4C+Al4C3 were also unsuccessful. Al3BC and Al4C3 phases form very easily and are observed in all samples even after short time sintering in contrast to Al3BC3, which forms very slowly at 900˚C. On the other hand Al3BC3 was always observed in arc melted samples containing 40–60 at.% Al and 10–30 at.% B. Experimental techniques for preparation concerned (a) melting of B4C in excess of Al for the synthesis of AlB40C4 (at 1550˚C, [1970Nei]), (b) melting of boron with excess of Al in a graphite crucible for synthesis of Al3B48C2 (at 1400˚C, [1964Mat]) (c) vapor deposition at 1400 to 1600˚C for single crystals of Al3B48C2 [1967Bli] (d) hot pressing of B4C+Al in graphite dies for synthesis of Al2.1B51C8 (at 1800˚C [1966Gie, 1966Lip]), (e) infiltration of B4C by liquid Al at 1100˚C and anneal at 1000˚C to obtain Al3BC [1987Sar], (f) reaction sintering of Al+B+C powder compacts on alumina boats in sealed silica capsules 627 to 1000˚C for the synthesis of Al3BC and phase relations at 1000˚C [1992Via, 1997Via] or at 1400˚C for 10 h for the production of the single crystals of Al3B48C2 [1994Kud] (g) melting of an Al8BC mixture in alumina under argon for 160 h at 850˚C and subsequent cooling at 150K/h to RT for production of black-bluish single crystals of Al3BC [1997Mey] (h) melting of an Al40B2C3 mixture in alumina under argon at 1500˚C and subsequent cooling at 10K/h to 600˚C for production of single crystals of Al3BC3 in the form of yellow, transparent platelets [1996Hil2] and (i) Al-flux solvent method for a general production of single crystals (see i.e. [1986Kis, 1990Oka, 1996Hil1]). Samples used for the isothermal section at 1400˚C were prepared from cold compacted powder mixtures of AlB2, B4C, B and/or C, which were reaction-sintered under Ar in closed Knudsen-type graphite reactors at 1600˚C for 1h prior to 48 h heat treatment at 1400˚C [1993Bau]. Phase relations at 900˚C were studied [2002Zhe] on elemental powder compacts sintered in alumina crucibles (binary Al-B alloys) or in closed graphite crucibles (ternary alloys). The specimens were sealed in evacuated quartz ampoules and were slowly heated for 10˚/h to 720˚C (slightly above the melting point of aluminium) and kept at this temperature for 48h. After temperature was increased to 900˚C at a rate of 20˚/h, the tablets were sintered at this temperature for 1 week. Repeated repowderisation (under protective cyclohexane) and sintering at 900˚C were necessary to reach equilibrium conditions. Several studies dealt with the kinetics of wetting of B4C surfaces by liquid aluminum; detailed discussions can be found in the articles by [1979Pan] and [1989Hal]. Hot-pressing of B4.3C+Al powders at 1820˚C, 45 MPa under Ar (5 to 20 mass% Al) revealed the formation of the ternary B4C- related Al-boron carbides (solution of Al in B4C, and τ2) although the products were all thought to belong to the B4C-based solid solution [2000Liu]. With increasing Al-content (>5 mass% Al) the Al3BC3 phase evolved [2000Liu]. DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
Thermodynamic calculations of the Al-B-C system have been attempted by [1982Doe, 1993Wen, 1993Kau], however, are not fully consistent with experimental observations. Reviews on the constitution and on the crystal structures of the Al-B-C system have been presented by [1977Mat, 1990Luk, 1998Rog].
Binary Systems The binary systems B-C and Al-C are consistent with the critical assessments of [1998Kas, 1996Kas] and [2003Per], respectively. In spite of numerous data available from literature on the constitution of the Al-B phase diagram, contradictory results exist for the formation of aluminium diboride (Table 1). Figure 1a shows the various versions for the Al-rich part of the Al-B phase diagram. It should be noted, that recent experiments [2002Zhe] confirmed the formation of AlB2 at 900˚C, in contrast to data of [1997Via] suggesting peritectic formation at 892 ± 5˚C. In the present assessment we accept the temperature of 956 ± 5˚C for the invariant reaction L+AlB12ÐAlB2 as determined by [2000Hal]. The adopted Al-B phase diagram (Figs. 1b, 1c) is based on the assessment of [1994Dus]. The composition of the peritectic liquid at 0.55 at.% B has been confirmed by a recent thermodynamic assessment of [2001Fje]. AlB2 is still taken as a stoichiometric compound in spite of the suggestions of [1964Mat, 1999Bur, 2002Bur] for Al-deficiency in terms of Al0.9B2. Although the assessment of [1994Dus] concluded a peritectic formation of AlB12, L+(B)Ð AlB12 at 2050˚C, the thermodynamic calculation of [1993Wen] is based on congruently melting AlB12 (TM = 2150˚C).
Solid Phases The crystallographic information on all the binary and ternary phases pertinent to the Al-B-C system is listed in Table 2. Some controversy exists in the crystallographic characterization of the modifications reported for Al3B48C2. A single crystal study [1995Hil, 1996Hil1, 2000Mey] on an untwinned specimen revealed a tetragonal high temperature form (closely related to the structure of I-tetragonal boron), which on cooling undergoes a symmetry reduction resulting in microscopically twinned products that hitherto were indexed on the basis of two orthorhombic modifications, labeled A and B by [1965Mat]. The transformation was earlier proposed to be at ca. 850˚C [1960Koh, 1965Mat], whereas new results from DTA recorded 650˚C [1996Hil1]. The transition seems to be rather fast, as the low temperature modification is present in samples furnace-cooled from 1400˚C to room temperature [1993Bau]. A second point of controversy concerns the phases AlB40C4 and Al2.1B51C8 for which detailed crystallographic descriptions are available, however, AlB40C4 actually being isotypic with binary B4C, hitherto is not thoroughly established as a ternary phase independent from binary B4C. As the two structurally closely related phases AlB40C4 and Al2.1B51C8 generally are found together, a high and low temperature transition between them may be inferred [1993Bau]. Without further details the maximum solid solubility of Al in boroncarbide (“B13C2”, at 1950˚C) was reported to be 1 mass% Al (equivalent to 2 at.% Al in B4C) [1978Ekb]. Experiments to establish a possible homogeneous range for Al3BC3 (earlier: “Al8B4C7” [1980Ino], or “Al4B1–3C4” [1964Mat]), were carried out at 1830˚C by [1980Ino] resulting in a Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
3
4
3
Al–B–C
rather stoichiometric composition without variation of the lattice parameters. These findings were confirmed by [1993Bau, 1996Hil2]. Details of the crystal structure with linear C-B-C chains are given by [1996Hil2]. Lattice parameters of Al3BC3 were measured at room temperature up to 7.5 GPa using a multi-anvil synchrotron system with B4C anvils; for a high temperature pressure experiment the sample was placed in a graphite ampoule [2000Sol]. Al3BC3 is free of structural transitions up to 1523˚C within the pressure range 2.5 to 5.3 GPa [2000Sol]. A further ternary compound τ5 was observed after infiltration by liquid Al at 1170˚C with post heat treatment for 100 h at 800 to 1000˚C [1987Sar]. The hexagonal lattice was established by TEM; the approximate composition “Al4BC” resulted from EELS-data [1987Sar]. This phase has been also confirmed by [1989Hal, 1990Pyz]. From a detailed investigation of this Al-rich boroncarbide by X-ray powder diffraction, LOM and EPMA, [1992Via] suggested a formula of Al3BC rather than “Al4BC” and attributed a hexagonal cell; additional weak lines in the X-ray intensity pattern of Al3BC prompted a larger unit cell pffiffiffi a = a0/ 3 [1993Gon]. Although the authors of [1997Mey] recognized the larger cell, the crystal structure of Al3BC was solved for the high symmetry subcell from single crystals isolated from a sample directly reacted from the elements - however, from EPMA a composition Al2.5BC was derived (see also Table 2). Al6B-octahedra and trigonal Al5C-bipyramids are the characteristic structural elements [1997Mey]. The various data on the compositional ranges of the τ4 and τ5 phases are summarized in Fig. 2. Half filled circles correspond to the accepted stoichiometries Al3BC and Al3BC3. From the significant change of the unit cell volume of Al4C3 comparing binary and ternary alloys, a solubility of boron is suggested [1996Bid, 2002Zhe, 2000Mey]. Solubility of boron in Al4C3 was established to be 3.4 at.% at 900˚C [2002Zhe] and an interesting behavior of lattice parameters was observed. In spite of the increase of the “a” parameter and of the cell volume with boron content, the “c” parameter decreases. That may be explained by a preferential distribution of boron and carbon atoms among different crystallographic sites. A significant solubility of boron in Al4C3 was also reported by [2000Mey] to be about 9.3 at.%, however, no details on the relevant temperature were given. Furthermore these authors claim for Al4C3–xBx lattice parameters increasing with boron content. Lattice parameters of Al4C3 for samples located in three-phase regions (Al)+Al4C3+Al3BC, Al4C3+Al3BC3+Al3BC and Al4C3+Al3BC3+(C) are very close, assuming that these three-phase regions meet at the Al4C3 phase at a maximal boron solubility of Al4(C0.92B0.08)3. Insignificant solubility of carbon in AlB2 is reported by [2002Zhe] comparing lattice parameters in ternary and binary samples; AlB2 with 0.5 at.% C, heat treated at 900˚C, already contains the Al3BC phase.
Isothermal Sections Phase equilibria for the 1400˚C isothermal section are summarized in Fig. 3, revealing the existence of four ternary compounds τ1 to τ4. A small field of liquid phase exists at 1400˚C which is in equilibrium with Al3B48C2, Al2.1B51C8 and with Al3BC3 [1993Bau]. Boron-poor equilibria agree with an earlier work by [1980Ino] who reported on the two-phase equilibria Al4C3+Al3BC3 (Al7B4C8), Al3BC3 (Al7B4C8)+B4C and Al3BC3 (Al7B4C8)+C. In Fig. 3 twophase equilibria are shown to exist between the binary solid solution “B4C” and AlB40C and Al2.1B51C8. At 1400˚C all ternary compounds seem to exist at their stoichiometric compositions [1993Bau], whilst [1965Eco] claimed a homogeneity range for τ1 at 1800˚C from DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
“AlB48C8” to Al3B48C8. Binary AlB12 was never seen in combination with Al2.1B51C8 nor with AlB40C4 [1993Bau]. The isothermal section at 1000˚C, Fig. 4, was constructed on the basis of data from [1997Via]. Due to low interaction kinetics in the boron- and carbon-rich part of the system at 1000˚C, equilibria in this portions of the diagram are preliminary. Moreover, ternary compounds τ1 and τ2 were not included in the 1000˚C section by [1997Via], τ4 was listed as “Al8B4C7”, and no solubility of boron in Al4C3 was considered. For consistency with the present knowledge on the Al-B-C system, the ternary compounds τ1 and τ2 were introduced in Fig. 4 and the composition of τ4 was changed to Al3BC3. The solubility of boron in Al4C3 at 1000˚C was estimated to be about 4 at.%, extrapolating from data of [2002Zhe] at 900˚C. Figure 5 represents the isothermal section at 900˚C [2002Zhe] confirming the equilibrium AlB2+Al3BC, whereas [1997Via] claimed this equilibrium to be only stable below 868 ± 4˚C. Similar to 1000˚C the equilibria at 900˚C involving τ1 and τ2 are not well established due to low reactivity of the components.
Invariant Equilibria, Liquidus Surface A tentative liquidus surface for the aluminum rich portion of the diagram (Fig. 6) was proposed by [1997Via], presenting equilibria involving the τ5 phase. The invariant equilibrium U5 (L+Al3B48C2ÐAlB2+Al3BC) was reported at 868 ± 4˚C by [1997Via], but this temperature can not be accepted in respect to the observed isothermal equilibrium AlB2+Al3BC at 900˚C [2002Zhe] suggesting such transformation above 900˚C. Comparison of the reaction scheme and the isothermal section at 1000˚C (Fig. 4) with the isothermal section at 1400˚C (Fig. 3) suggests a rather complicate picture of the phase transformations in this regions mainly due to decomposition of τ5. Based on an earlier thermodynamic calculation by [1982Doe], a reaction scheme was derived [1990Luk], which gives a tentative information of the solidification behavior in the AlB-C ternary. The temperatures of the invariant equilibria were estimated and the ternary compounds τ1 to τ3 were assumed to be part of the solid solution arising from binary B4C; τ5 was not included. A more recent thermodynamic modelling of the Al-B-C phase diagram by [1993Wen] as part of the multi-component Al-B-C-N-Si-Ti system treated the ternary compounds τ1, τ2, τ3 as independent phases, however, the peritectoid formation of τ4 (Al3BC3) is in strict contradiction to the experimentally confirmed two-phase equilibrium τ4+τ5 (Al3BC3+Al3BC) [1997Via, 2002Zhe] as well as to the observed existence of τ4+τ5 in as cast alloys [2002Zhe], thereby strongly indicating direct formation of Al3BC3 from the liquid. A closed ternary miscibility gap in the Al-rich liquid is suggested from thermodynamic calculations by [1993Kau], however, hitherto without experimental confirmation [2002Zhe]. Figure 7 presents a reaction scheme for the major parts of the Al-B-C phase diagram. The reaction scheme is essentially based (i) on the tentative liquidus projection for the Al-rich part as suggested by [1997Via], (ii) on the experiments of [2002Zhe] concerning the solidification of the phases τ4, τ5 and (iii) on the thermodynamic calculation of [1993Wen] for the B-rich part, however, accepting peritectic formation of AlB12.
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
5
6
3
Al–B–C
Thermodynamics Enthalpies of formation and heat capacity measurements from a Calvet type automatic microcalorimeter in the temperature range 310–1200 K were reported by [1987Kis] and are listed as follows: Al3 B48 C2 : H 0 ðTÞ H 0 ð298Þ ¼ 0:7945 103 T 2 þ 0:5182T 225:1374 ðin J g1 Þ and Cp ðTÞ ¼ 0:1589 102 T þ 0:5182 ðJ g1 K1 Þ Al2:1 B51 C8 : H 0 ðTÞ H 0 ð298Þ ¼ 0:7226 103 T 2 þ 0:5411T 225:5702 1
ðin J g
:
for AlB24 C4 Þ and
Cp ðTÞ ¼ 0:1589 102 T þ 0:5182 ðJ g1 K1 for AlB24 C4 Þ Thermodynamic calculations of the Al-B-C system due to [1982Doe, 1993Wen, 1993Kau], however, are not fully consistent with experimental observations. For detailed discussion, see section Invariant Equilibria.
Notes on Materials Properties and Applications Mechanical properties of Al-B4C cermets and boron/carbon fiber-aluminium composites have been investigated by various groups [1972Bak, 1973Her, 1975Mun, 1984Via, 1985Che, 1985Hal, 1985Kov, 1985Pyz, 1985Sar, 1986Che, 1986Dub,1990Ram, 1996Pyz, 2002Ars]; the effect of reaction on the tensile behavior of infiltrated composites was reported by [2002Kou2] and size dependent strengthening in particle reinforced Al by [2002Kou1]; reaction products were studied by [2001Lee]. An increase of surface hardness of about 25 to 40 % can be achieved by impulse laser radiation on B4C/Al cermets [1988Kov]. Wetting of B4C by Al has been studied by many research teams with rather contradicting results, until the temperature and time dependent occurrence of chemical reactions/compound formation was analyzed in detail (for discussion see i.e. [1979Kis, 1979Pan, 1989Hal, 2000Kha]). The kinetics of wetting by liquid aluminium of flat, sintered boron carbide specimens with residual porosity less than 3 % were investigated by [1979Pan]. The speed of spreading of liquid aluminium at 1100˚ to 1200˚C was measured to be 0.1–0.8 mm·s–1, in accordance with r2 = f(t), where r equals the radius of the contact circle. The angle of contact was first 92˚, however, in 3 to 5 min decreased to 28˚. The slow spreading was determined by the formation of new aluminum boron carbide phases in the contact zone with a microhardness of ca. 13 GPa. The driving force Δσ = σ (cos Θ0-cosΘ) (σ = surface tension of the melt, Θ0 = contact angle of the melt, Θ = contact angle at time (t)) decreased sharply becoming zero in 4 to 5 min [1979Pan]. The contact angle of molten Al on B4C as a function of processing time for various isotherms at 5·10–3 to 10–4 Pa was also given by [1989Hal] based on sessile drops cooled to room temperature. Mechanical properties, electrical and thermal conductivity as well as their temperature dependencies were reported on the Knoop and Vickers microhardness for Al-flux grown (temperature region 1750 to 800˚C) ‘‘amber’’ single crystals Al3B48C2 and for ‘‘black’’ crystals (αAlB12, γAlB12 and AlB2.1B51C8) [1986Kis]. These studies were also performed on hot pressed specimens of various compositions x(AlB12)+(1–x)B4C and Al3B48C3 in the temperature range 24 to 827˚C [1991Kha1, 1991Kha3]. For Al3BC3 (“Al8B4C7”), Al3B48C3, Al2.1B51C8 [1991Kha2] DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
also examined these properties as a function of porosity and quantity of Fe-impurity. These data are summarized in Table 3 including information on flux-grown crystals Al3B48C2 and Al2.1B51C8 [1990Oka]. Both types of crystals were said to be p-type semiconductors [1986Kis]. In a ring test the strength of a powder compact of B13C2 +1 mass% Al, sintered at 1950˚C, was found to be 0.50(7) GNm–2 [1978Ekb]. [1991Kha2] reported on the kinetics of thermal densification of hot pressed powders of B4C, AlB12, Al3B48C2 and Al3BC3. Kinetics of dissolution in HCl, HNO3 and HCl-HNO3 was studied by [1998Kha] as well as the resistance of Al-boron carbides to alkali and hydrogen peroxide. [1989Hal] studied the densification kinetics of Al+B4C cermets in the range from 800 to 1400˚C in pressureless sintering as well as after applying hot isostatic pressure. The kinetic of metal depletion in post heated dense cermets B4C/Al at temperatures between 600˚C and 1000˚C was investigated by [1990Pyz]. Chemical stability against various boiling acids, oxidation resistance, IR and EPR spectra of Al-borides and Al-boron carbides (Al3B48C2, Al2.1B51C8) was studied by [1991Pri]. The spectra were taken at 77 K and 300K and for different crystal orientations relative to the magnetic field. Absorption edge and IR-active phonons in Al3B48C2 were reported by [1987Hau, 2000Wer] and IR spectra of boron carbide containing up to 1.5 at.% Al were determined between of 8 to 500 mm–1 wave numbers and for temperatures between 70 to 450 K [1997Sch]. These data seem to suggest the incorporation of Al-atoms into binary boroncarbide in form of pairs substituting the B-B-C or C-B-C chains [1997Sch]. Characteristic IR absorption bands for finely dispersed powders of Al-borides and Al-boron carbides were listed by [1998Kha]. The Seebeck-coefficients were reported to linearly increase from 260 μVK–1 for binary “B4C” to 450 μVK–1 for 1.4 at.% Al dissolved, revealing p type behavior [1997Sch]. Seebeckcoefficients, thermal and electric conductivities were further reported by [2000Liu] for B4.3Cbased samples containing 0.5, 10, 15, 20 mass% Al, highlighting the Z-value at RT of 1.04·10–6K–1 for the 5 mass% Al sample. IR and Raman spectroscopy on Al3BC3 (at RT) confirm the linear (CBC)5– unit as an isoelectronic CO2-analogon [1996Hil2, 2000Mey]. On heating in air, Al3BC3 (earlier reported as Al8B4C7), Al3B48C3 and Al2.1B51C8 show low oxidation at 500˚C (increase of mass 4 mgh–1); intensive oxidation, with a mass increase of 40 mgh–1) starts at 1280˚C for Al2.1B51C8 and at 1370˚C for Al3B48C2 [1991Pri, 1989Kha, 1991Kha4]. Oxidation in air of single crystals Al2.1B51C8 and Al3B48C2 started at about 760˚C and 710˚C, respectively [1990Oka]. The reaction products were 9Al2O3·2B2O3 for Al2.1B51C8 crystals and B2O3 for AlB40C4 specimens [1994Kud]. Whereas Al3BC3 was said to be unstable in acids [1991Kha4], more detailed experiments [1996Hil2] proved stability at room temperature against bases and dilute acids, except for HNO3 and HF. Al3BC3 was furthermore said to be stable in air up to 600˚C [1991Kha4,1996Hil2]. Al3BC is quickly attacked by dilute HCl [1997Mey]. Thermophysical properties of sintered bodies of Al3BC3 have been derived by [2000Wan]. These are linear thermal expansion in the range of 25 to 1200˚C, specific heat and thermal diffusivity via laser flash technique, Youngs modulus of 136.6 GPa, Vickers hardness of 12.1 GPa at a load of 196 N and thermogravimetric recording of growth of an oxidized layer on heating in air up to 1500˚C. Fitting a Birch-Murnaghan equation of state to the pressure dependency of the lattice parameters of Al3BC3 up to 7.5 GPa, the isothermal bulk modulus was B0 = 153 ± 6 GPa (dB0/ dp = 19 ± 4) [2000Sol]. Despite high bulk modulus the Vickers hardness of single crystals is as low as 20.7 GPa at a load of 25g and 18.2 GPa at a load of 50g [2000Sol]. Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
7
8
3
Al–B–C
Al3BC was successfully prepared by self propagating high temperature synthesis induced by mechanical activation of Al-B-C powder mixtures in air; mixtures low in boron (AlB0.1C) resulted in Al3BC3 under violent emission of heat [1999Tsu]. In contrast to that [2000Sav] was unable to prepare ternary aluminoborocarbides from mechanochemical synthesis. Elastic bulk and shear moduli for Al3BC (earlier reported as Al4BC) were measured by [1995Pyz] and estimated by [1999Tor].
Miscellaneous A series of patents covers the techniques to produce dense B4C/Al cermets by infiltration of the metal matrix into the porous ceramic body without wetting reactions [1976Lan, 1986Hal, 1987Pyz, 1990Pyz, 1991Pyz, 1995Pyz, 1996Pyz, 1997Du , 2000Pyz, 2001Lee]; subsequent heat treatment results in materials with designed chemistry and microstructures, flexure strength, hardness and fracture toughness. Fine microstructures were obtained via ultrarapid microwave heating [1995Rug]. B4C/Al cermets have been considered as an improved structural neutron absorber [1977Ros, 1978Boi, 1978Sur, 1986Ros, 1987Lev, 1992Bei] and for applications as friction materials for automotive brake applications [1999Cha]. Oxidation protective B4C-coatings on C-fibers in Al-matrix were reported by [1996RMi] and [1996Vin] produced C-fibres-Al composites by a squeeze casting technique. Explosive consolidation to produce Al/ B4C composites was studied by [1995Bon, 1997Yue]. Shock recovery experiments were performed on a 65 vol% B4C-Al cermet as a function of shock pressure [1989Blu].
. Table 1 Literature Data on Experimental Temperatures of Invariant Equilibrium L+AlB12ÐAlB2 T [˚C]
Technique
Heating Rate
References
Stability observation
-
1000 - 1500
[1936Hof]
Synthesis observation
-
980
[1967Ser]
DTA
4˚C/min
920
[1967Ato]
Stability observation
-
1350 - 1500
[1972Sir]
DTA
5˚C/min
1030 ± 5
[1993Ips]
Synthesis observation
-
892 ± 5
[1997Via]
DSC and Stability observation
0˚C/min*
956 ± 5
[2000Hal]
DSC
10˚C/min
914 ± 55
[2001Fje]
* DSC measurements were performed with heating rate of 5, 15 and 40˚/min., and extrapolated to 0˚C/min.
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
. Table 2 Crystallographic Data of Solid Phases
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
(Al) < 660.452
cF4 Fm3m Cu
a = 404.96
[Mas2 ]
(βB) < 2092
hR333 R3m βB
a = 1093.30 c = 2382.52 a = 1092.2 c = 2381.1 a = 1096.5 c = 2386.8 a = 1097.4 c = 2387.7
[Mas2 , 1993Wer]
a = 246.12 c = 670.90 a = 246.023 c = 671.163 a = 246.75 c = 669.78
[Mas2 ]
(C) < 3827 (B.P.)
B4C < 2450
hP4 P63/mmc C-graphite
hR45 R3m B13C2
at 1.1 at.% C [1993Wer] linear da/dx, dc/dx at AlB31 [V-C2 ] from sample Al4B95C1, quenched from 1400˚C, contains Al3B48C2 and αAlB12 [1993Bau]
[1967Low] at 2.35 at.% Bmax (2350˚C) linear da/dx, dc/dx, [1967Low]
a = 565.1 c = 1219.6 a = 560.7 c = 1209.5 a = 560.3 c = 1209.8
from sample containing τ2, τ4, quenched from 1400˚C [1993Bau]
9 to 20 at.% C [1990Ase]
B25C
tP52 P42m B25C
a = 872.2 c = 508.0
[V-C2 ] also B51C1, B49C3; all metastable?
Al2B3 ≤ 525
hR* Al2B3 (?)
a = 1840 c = 896
at 60 at.% B [1992Var] metastable?
AlB2 ≤ 956±5
hP3 P6/mmm AlB2
a = 300.6 b = 325.2 a = 300.67 ± 0.01 b = 325.36 ± 0.02 a = 300.63 ± 0.01 b = 325.46 ± 0.01 a = 300.43 ± 0.03 b = 325.19 ± 0.06
[1994Dus], temperature from [2000Hal] [2002Zhe]
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
[2002Zhe] in 33.3Al-66.2B-0.5C, in equilibrium with τ5 at 900˚C [1999Bur] for Al0.9B2
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
9
10
3
Al–B–C
. Table 2 (continued)
Phase/ Temperature Range [˚C] αAlB12 ≤ 2050
γAlB12
Pearson Symbol/ Space Group/ Prototype tP216 P41212 αAlB12
oP384 P212121 γAlB12
Lattice Parameters [pm] a = 1015.8 c = 1427.0 a = 1018 c = 1434.3 a = 1016.3 c = 1425.6 a = 1015.5 c = 1426.0 a = 1014.93 ± 0.07 c = 1425.0 ± 0.5 a = 1014.4 b = 1657.3 c = 1751.0
hR21 R 3m Al4C3
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
[1994Dus] ρexp. = 2.65 Mgm–3 [1991Pri] from sample Al2B92C2, quenched from 1400˚C, contains Al3B48C2 [1993Bau] from sample Al4B95C1, quenched from 1400˚C, contains Al3B48C2 and AlB31 [1993Bau] [2002Zhe] [1983Hig, 1994Dus, 2000Hig] metastable phase or ternary product stabilized by small amounts of impurity metals present in Alflux grown material ρexp. = 2.56 Mgm–3 [1991Pri]
a = 1019.5 b = 1666 c = 1769 Al4C3 < 2156
Comments/References
a = 333.8 c = 2511.7 a = 334.21 ± 0.01 c = 2503.2 ± 0.5 a = 335.78 ± 0.02 c = 2499.6 ± 0.5
MSIT1
[2003Per, V-C2 ] [2002Zhe] [2002Zhe] in 57.1Al-4.3B-38.6C Al4(C0.9B0.1)3, in equilibrium with τ5 at 900˚C
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
. Table 2 (continued)
Phase/ Temperature Range [˚C] * τ1, Al2.1B51C8 (eventually low temperature phase of τ2)
* τ2, AlB40C4 (eventually high temperature phase of τ1)
Pearson Symbol/ Space Group/ Prototype oC88 Cmcm Al2B51C8
hR45 R3m B4C-deriv.
Lattice Parameters [pm]
earlier labeled “AlB10” [1967Wil] or AlB24C4 [1964Mat, 1969Wil, 1970Wil] [1969Per] ρexp. = 2.54 Mgm–3
a = 569.0 b = 888.1 c = 910.0 a = 568.7 b = 887.7 c = 909.8 a = 569.0 b = 888.1 c = 910.0 a = 569.3 b = 884.7 c = 909.3 a = 567.6 b = 891.4 c = 909.5 a = 569.2 b = 889.2 c = 911.2
from sample containing τ2 and τ3, quenched from 1400˚C [1993Bau] from sample containing τ4, quenched from 1400˚C [1993Bau] from sample Al4B92C4 quenched from 1400˚C, contains Al3B48C2 (tetragonal), Al3B48C2 (A) and AlB40C4 [1993Bau] [1991Pri]
[1990Oka] ρexp. = 2.54 Mgm–3 single crystals from Al-flux
a = 564.2 c = 1236.7 a = 565.37 c = 1231.4 a = 564.8 c = 1239.9 a = 565.6 c = 1238.9
[1970Nei] ρexp. = 2.52 Mgm–3 from sample containing τ1, τ3, quenched from 1400˚C [1993Bau] from sample containing τ4 and B4C, quenched from 1400˚C [1993Bau] from sample Al4B92C4 quenched from 1400˚C, contains also Al3B48C2 (tetrag.), Al3B48C2 and Al2.1B51C8 [1993Bau] [1966Gie] for composition “Al2B48C8”
a = 563 c = 1129 a = 565 c = 1239
Landolt‐Bo¨rnstein New Series IV/11E1
Comments/References
[1966Lip] for composition “Al4B48C8”
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
11
12
3
Al–B–C
. Table 2 (continued)
Phase/ Temperature Range [˚C] * τ3, Al3B48C2 (r) < 650
Pearson Symbol/ Space Group/ Prototype oI212 Imma Al3B48C2
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
Lattice Parameters [pm] a0 = 1240.7 b0 = 1262.3 c0 = 1014.4 a = 1234 b = 1263 c = 508 a = 1232.5 b = 1261.4 c = 1016.2 a = 1233.72 b = 1262.41 c = 1016.06 a = 1232.5 b = 1264.7 c = 1016.2 a = 1230.2 b = 1262.1 c = 1016.1 a = 1229.1 b = 1262.2 c = 1015.88 a = 1233.62 b = 1262.40 c = 1015.94 a = 1239.0 ± 0.3 b = 1263.7 ± 0.3 c = 1013.6 ± 0.4 a = 1237.7 b = 1262.7 c = 507.9 to a = 1236.3 b = 1261.6 c = 510.2 a = 616.6 b = 1263.5 c = 1065.6 a = 618.1 b = 1262.2 c = 1016.1 a = 617 b = 1263 c = 1016
MSIT1
Comments/References [1996Hil1], only one low temperature modification! [1965Mat], two modifications, microscopically twinned; modification A, c = c0/2 from a sample Al6B92C2 cooled from 1400˚C contains “AlB12” [1993Bau] from sample Al4B95C1 cooled from 1400˚C contains also “AlB12”, AlB31 [1993Bau] [1991Pri]
[1994Kud]
from sample Al4B92C4 cooled from 1400˚C, [1993Bau] contains Al2.1B51C8, AlB40C4 and tetragonal Al3B48C2 [1993Bau] from sample Al4B95C1, cooled from 1400˚C, see above. [2000Wer]
[1990Oka] single crystals from Al-flux modification A ; c = c0/2
[1990Oka] single crystals from Al-flux ρexp. = 2.59(2) Mgm–3 modification B, a = a0/2
[1965Mat] modification B a = a0/2
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
. Table 2 (continued)
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm] a = 616.4 b = 1262.1 c = 1016.4
* τ3, Al3B48C2 (h) > 650
* τ4, Al3BC3 < 1835
*τ5, Al3BC < 1100
[1991Pri] a = a0/2
tP52 a = 885 P42/nnm c = 508 B25C -deriv. a = 882 c = 509 a = 881.9 c = 508.25 hP42 P3c1a) Mg3BN3
hP20 P3c1 (P63/mmc for subcell) Al3BC
Comments/References
[1996Hil1] high temperature modification [1965Mat] from sample Al4B92C4 cooled from 1400˚C, contains also Al2.1B51C8, AlB40C4 and orthorhombic Al3B48C2 [1993Bau]
a = 589.97 c = 1589.0 a = 590.6 c = 1590.1 a = 590.7 c = 1591.3 a = 590.5 c = 1590.5 a = 340.1 ± 0.3 c = 1584 ± 0.2 a = 590.22 ± 0.3 c = 1589.4 ± 0.1 a = 605.0 c = 1154.0 a = 603.45
[1996Hil2] ρ = 2.66 Mgm–3 temperature from [1980Ino] [1980Ino], labelled as Al8B4C7 from sample containing τ1, quenched from 1400˚C [1993Bau] from sample containing τ2 and B4C, quenched from 1400˚C [1993Bau] pffiffiffi [2000Sol], subcell with a = a0/ 3 pressure dependence of the lattice parameters is given up to 7.5GPa [2002Zhe] [1993Gon, 1997Via]
c = 1152.02 a = 6041.9 ± 0.2 c = 1154.0 ± 0.3 a = 349.1 c = 1154.1 a = 352.0 c = 582.0
[1997Mey] from single crystals, “Al2.5BC” from EPMA [2002Zhe] pffiffiffi [1992Via], subcell with a = a0/ 3 [1987Sar], earlier “Al4BC” subcell with a = a0/ p ffiffiffi 3, c = c0/2
pffiffiffi P63/mmc for subcell with a = a0/ 3, c = c0
a)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
13
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
(101)
(001)
γAlB12
(100)
(111)
(100)
(111)
αAlB12
Al3BC3
Al2.1B51C8
Al3B48C2
29.6(1.0) 25.8(7) 22.8(8) 21.6(1.1)
19.6(5)
22.6 26 6 24.2(7) 25.0–26.9
37.6(2.0) 31.7(8) 23.7(6)
27.1(5)
26.5(5) 23.1
(0.5N, 293K) (1N, 293K) (2N, 293K) (4.9N, 293K)
(2N, 293K)
(2N, 293K) (5N, 293K) (5N, 1200K) (2N, 293K) (1N, 293K)
(0.5N, 293K) (1N, 293K) (4.9N, 293K)
(2N, 293K)
(2N 293K) (5N, 293K)
34.4(2.7) 31.0(1.5) 27.3(1.2) 23.8(9)
20.7 18.2
25.7 to 30.5
(0.5N, 293K) (1N, 293K) (2N, 293K) (4.9N, 293K)
(0.25N, 293K) (0.50N, 293K)
(1N, 293K)
33.6(1.6) (2N, 293K)
1.8(2)
1.5(3)
2.7(2)
5.3 4(1)
Fracture Toughness K1c [MPa·m1/2]
0.1
1 0.6 - 1.2
0.18 - 0.36
3.85 · 105 0.22
5.92 ·102
2.02 · 105 0.08 - 0.18
10–3 - 1
104-106 2.6·10310–6 2.6·10–6
ρ293K [Ωm]
Activation Energy ΔE [eV] 100K to 400K R=R0exp(-ΔE/2kT)
38.7 (310K) 60 (600K)
19.6 (310K)
Thermal Conductivity [Wm–1K–1]
[1986Dub] [1986Dub] [1991Pri] [1986Dub]
[1991Pri]
[2000Sol]
[1986Kis] [1986Kis] [1986Kis] [1991Pri] [1990Oka]
[1990Oka, 1994Kud] [1986Dub] [1986Dub] [1986Dub]
[1986Kis] [1986Kis] [1986Kis] [1991Pri]
References
3
Microhardness [GPa] at Various Loads and Temperatures Crystal Face Vickers Compound of Indent Knoop
. Table 3 Microhardness, Fracture Toughness, Electrical Conductivity, Activation Energies for Electrical Conductivity and Thermal Conductivity for Various Aluminium Borides and Aluminium Boron Carbides
14 Al–B–C
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
. Fig. 1a Al-B-C. Various versions of the Al-rich part of the Al-B diagram
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
15
16
3
Al–B–C
. Fig. 1b Al-B-C. Accepted Al-B phase diagram
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
. Fig. 1c Al-B-C. Accepted Al-B phase diagram, enlarged Al-rich region
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
17
18
3
Al–B–C
. Fig. 2 Al-B-C. Superposition of literature data on the homogeneity regions of τ4 and τ5 phases. Halffilled circles correspond to the accepted compositions
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
. Fig. 3 Al-B-C. Isothermal section at 1400˚C; the position of Al3BC is indicated by a full circle
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
19
20
3
Al–B–C
. Fig. 4 Al-B-C. Isothermal section at 1000˚C
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C
3
. Fig. 5 Al-B-C. Isothermal section at 900˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
21
22
3
Al–B–C
. Fig. 6 Al-B-C. Tentative liquidus surface projection
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
3
. Fig. 7 Al-B-C. Reaction scheme
Al–B–C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
23
24
3
Al–B–C
References [1936Hof] [1960Koh] [1963Wil] [1964Mat] [1965Eco] [1965Mat] [1966Gie] [1966Lip] [1967Ato] [1967Bli] [1967Low] [1967Ser] [1967Wil] [1969Per] [1969Wil] [1970Nei] [1970Wil] [1972Bak] [1972Sir] [1973Her]
[1975Mun]
[1976Lan]
[1976Mon] [1977Mat] [1977Ros]
Hofmann, W., Jaeniche, W., “Contribution to the Knowledge of the Aluminium-Boron System” (in German), Z. Metallkd., 1, 1–5 (1936) (Phase Diagram, Crys. Structure, 13) Kohn, J.A., Eckart, D.W., “Aluminium Boride, AlB12”, Anal. Chem., 32, 296–298 (1960) (Crys. Structure, Experimental, 6) Will, G., “On the Crystal Structure of AlB10”, J. Am. Chem. Soc., 85, 2335–2336 (1963) (Crys. Structure, Experimental; 7) Matkovich, V.I., Economy, J., Giese Jr. R.F., “Presence of Carbon in Aluminium Borides”, J. Am. Chem. Soc., 86, 2337–2340 (1964) (Crys. Structure, Experimental, 14) Economy, J., Matkovich, V.I., Giese, Jr.R.F., “Crystal Chemistry of α-Boron Derivatives”, Z. Kristallogr., 122, 248–258 (1965) (Review, Crys. Structure, 26) Matkovich, V.I., Giese, Jr.R.F., Economy, J., “Phases and Twinning in C2Al3B48”, Z. Kristallogr., 122, 108–155 (1965) (Crys. Structure, Experimental, 7) Giese, Jr.R.F., Economy, J., Matkovich, V.I., “Topotactic Transition in C4AlB24”, Acta Crystallogr., 20, 697–698 (1966) (Crys. Structure, Experimental, 7) Lipp, A., Ro¨der, M., “On an Aluminium Bearing Boron Carbide” (in German), Z. Anorg. All. Chem., 343, 1–5 (1966) (Crys. Structure, Experimental,13) Atoda, T., Higashi, I., Kobayashi, M., “Process of Formation and Decomposition of Aluminium Borides”, Sci. Papers Inst. Phys. Chem. Res., 61, 92–99 (1967) (Phase Diagram, Crys. Structure, 8) Bliznakov, G., Peshev P., Niemyski, T., “On the Preparation of Crystalline Aluminium Borides by a Vapour Deposition Process”, J. Less-Common Met., 12, 405–410 (1967) (Experimental, 14) Lowell, C.E., “Solid Solution of Boron in Graphite”, J. Am. Ceram. Soc., 50, 142–144 (1967) (Crys. Structure, Experimental, 5) Serebryanskii, V.T., Epel’baum, V.Z., Zhdanov, G.S., “Equilibrium Diagram of the Aluminium - Boron System”, Russ. J. Inorg. Chem., 12(9), 1311–1316 (1967) (Phase Diagram, 33) Will, G., “Crystal Structure Analysis of AlB10 by the Convolution Molecule Method”, Acta Crystallogr., 23, 1071–1079 (1967) (Crys. Structure, 11) Perrotta, A.J., Townes, W.D., Potenza, J.A., “Crystal Structure of C8Al2.1B51”, Acta Crystallogr., 25B, 1223–1229 (1969) (Crys. Structure, Experimental, 11) Will, G., “The Crystal Structure of C4AlB24”, Acta Crystallogr., 25B, 1219–1222 (1969) (Crys. Structure, Experimental, 11) Neidhard, H., Mattes, R., Becher, H.J., “On the Preparation and Structure of an Aluminium Bearing Boron Carbide”, Acta Crystallogr., 26B, 315–317 (1970) (Crys. Structure, Experimental, 11) Will, G., “On the Existence of AlB10: a Critical Review of the Crystal Structures of AlB10 and C4AlB24”; Electrochem. Technol., 3(1-2), 119–126 (1970) (Crys. Structure, Experimental, 11) Baker, A.A., Braddick, D.M. Jackson, P.W., “Fatigue of Boron-Aluminium and Carbon-Aluminium Fibre Composites”, J. Mater. Sci., 7, 747–62 (1972) (Mechan. Prop., Experimental, 18) Sirtl, E., Woerner, L.M., “Preparation and Properties of Aluminium Diboride Single Crystals”, J. Cryst. Growth, 16, 215–218 (1972) (Crys. Structure, Phase Diagram, 15) Herring, H.W., Lytton, J.L., Steele, J.H., “Experimental Observations of Tensile Fracture in Unidirectional Boron Filament Reinforced Aluminium Sheet”, Metall. Trans. A, 4(3), 807–817 (1973) (Experimental, Mechan. Prop., 9) Munir, Z.A., Veerkamp, G.R., “Investigation of the Parameters Influencing the Microstructure of HotPressed Boron Carbide”, California Univ., Davis (USA). Dept. of Engineering,. 95 pp. (1975) (Mechan. Prop., Crys. Structure, 32) Lange, R.G., Munir, Z.A., “Sintering Kinetics of Pure and Doped Boron Carbide. Final Technical Report”, California Univ., Davis (USA). Dept. of Mechanical Engineering, 35 pp. (1976) (Experimental, 0) Mondolfo, L.F., “Aluminium - Boron System” in “Aluminium Alloys: Structure and Properties”, Butterworths, London, pp. 228–230 (1976) (Review, Phase Diagram, 29) Matkovich, V.I., Economy, J., “Structural Determinants in Higher Borides” in “Boron and Refractory Borides”, Matkovich, V.I. (Ed.), Springer Verlag, Berlin, 78–95 (1977) (Crys. Structure, Review, 36) Roszler, J.J., “Production of Neutron Shielding Material. Patent; B4C+Al in Al Boxes”, US Patent Document 4,027,377/A/, (1977)
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C [1978Boi]
[1978Ekb] [1978Sur] [1979Kis]
[1979Pan]
[1980Ino] [1982Doe]
[1983Hig] [1984Sig] [1984Via] [1985Che]
[1985Hal]
[1985Kov]
[1985Pyz]
[1985Sar]
[1986Che] [1986Dub] [1986Hal] [1986Kis] [1986Pes]
[1986Ros] [1987Hau]
3
Boiko, Yu.V., Gol’tsev, V.P., Gorobtsov, V.G., Kavkhuta, G.A., Strelkov, G.I., Khrenov, O.V., Yuzhanin, M.I., “Development and Investigation of Properties of Disperse Boron-Containing Materials for Control Rods of a Nuclear Reactor” (in Russian), Vest. Akad. Navuk BSSR, Ser. Fiz.-Energ. Navuk, 3, 5–8 (1978) (Mechan. Prop., Experimental) Ekbom, L.B., “Effect of Increased Boron Content on the Sintering Behavior and Mechanical Properties of Boron Carbide”, Keram. Z., 183–189 (1978) (Experimental, Mechan. Prop., 6) Suri, A.K., Gupta, C.K., “Studies on the Fabrication of Aluminium Bonded Boron Carbide Rings”, J. Nucl. Mater., 74(2), 297–302 (1978) (Experimental, 4) Kislyi, P.S., Kozina, G.K., Bodnaruk, N.I., “Wetting and Impregnation of Boron Carbide with Copper, Aluminum, and Their Alloys” (in Russian), Adgez. Rasplav. Pajka Mater., 4, 54–57 (1979) (Experimental) Panasyuk, A.D., Oreshkin, V.D., Maslennikova, V.R., “Study of the Kinetics of the Reactions of Boron Carbide with Liquid Aluminium, Silicon, Nickel and Iron”, Sov. Powder Metall. Met. Ceram., 199(7), 487–490 (1979), translated from Poroshk. Metall., 199(7), 79–83 (1979) (Experimental, 9) Inoue, Z., Tanaka, H., Inomata, Y., “Synthesis and X-Ray Crystallography of Aluminium Boron Carbide”, J. Mater. Sci., 15, 3036–3040 (1980) (Crys. Structure, Experimental, 7) Do¨rner, P., “Constitutional Investigations on High Temperature Ceramics of the B-Al-C-Si-N-O System by Means of Thermochemical Calculations” (in German), Thesis, Univ. Stuttgart (1982) (Experimental, Thermodyn., 126) Higashi, I., “Aluminum Distribution in the Boron Framework of γ-AlB12”, J. Solid State Chem., 47, 333–349 (1983) (Crys. Structure, 17) Sigworth, G.K., “The Grain Refining of Aluminium and Phase Relationships in the Al-Ti-B System”, Mater. Trans. 15A, 277–282 (1984) (Experimental, Phase Diagram, Thermodyn. Calculation, 28) Viala, J. C., Bouix, J., “Elaboration of Aluminum-Matrix Composite Materials Reinforced with Inorganic Fibers”, Mater. Chem. Phys., 11(2), 101–123 (1984) (Mechan. Prop., Experimental, 41) Chernyshova, T.A., Tsirlin, A.M., Gevlich, S.O., Rebrov, A.V., Obolenskii, A.V., “Effect of Surface Condition on the Strength of Coated Boron Fibers”, Sov. Powder Metall. Met. Ceram., 24(3), 210–213 (1985), translated from Poroshk. Metall., 24(3), 39–43 (1985) (Mechan. Prop., Experimental, 9) Halverson, D.C., Pyzik, A.J., I.A. Aksay, I.A., “Processing and Microstructural Characterization of B4CA1 Cermets”, “Composites and Advanced Ceramic Materials”, Anon. Proc. 9th Annu. Conf., American Ceramic Society, Inc., Columbus, OH, 736–744 (1985) (Mechan. Prop., Experimental, 14) Koval’chenko, M.S., Laptev, A.V., Zhidkov, A.B., “Annealing Effect on Structure and Properties of Hot Pressed Cermets Based on Boron Carbide” (in Russian), Poroshk. Metall., 24(9), 51–54 (1985) (Mechan. Prop., Experimental, 6) Pyzik, A. J., Aksay, I. A., “Processing, Microstructure, and Mechanical Properties of Boron CarbideAluminum Alloys Composites”, Anon. Abst. 38th Annu. Pacific Coast Regional Meeting American Ceramic Society, American Ceramic Society, Columbus, OH, (1985) (Mechan. Prop., Experimental, 0) Sarikaya, M., Pyzik, A.J., Ilsay, I.A., Snowden, W. E., “Effect of Secondary Phases on the Properties of B4C-A1 Composites.”, Anon. Abst. of the 38th Annu. Pacific Coast Regional Meeting American Ceramic Society, American Ceramic Society, Columbus, OH, (1985) (Mechan., Prop., Experimental, 0) Chernyshova, T.A., Rebrov, A.V., “Interaction Kinetics of Boron Carbide and Silicon Carbide with Liquid Aluminium”, J. Less-Common Met., 117, 203–207 (1986) (Kinetics, Experimental, 4) Dub, S.N., Prikhna, T.A., Il’nitskaya, O.N., “Mechanical Properties of the Al-B-C Compounds Crystals” (in Russian), Sverkhtverd. Mater., 6, 12–18 (1986) (Mechan. Prop., Experimental, 22) Halverson, D.C., Pyzik, A.J., Aksay, I.A., “Boron-Carbide-Aluminum and Boron-Carbide-Reactive Metal Cermets”, US patent document 4,605,440/A/, (1986) Kisly, P.S., Prikhna T.A., Golubyak, L.S., “Properties of High-Temperature Solution Grown Aluminium Borides”, J. Less-Common Met., 117, 349–353 (1986) (Experimental, 10) Peshev, P., Gyurov, G., Khristov, M., Gurin, V.N., Korsukova, M. M., Solomkin, F.Yu., Sidorin K.K., “Preparation and some Properties of Aluminium Carboboride Single Crystals”, J. Less-Common Met., 117, 341–348 (1986) (Crys. Structure, Mechan. Prop., Optical Prop., Experimental, 16) Roszler, J.J., “Process for the Manufacture of a Material Shielding Against Neutrons” (in German), DE Patent Document 2643444/C2/, (1986) Haupt, H., Werheit, H., Siejak, V., Gurin, V.N., Korsukova, M.M., “Absorption Edge and IR-active Phonons of Al3B48C2, “Boron, Borides and Related Compounds”, Proc. 9th Int. Sympos., Werheit, H. (Ed.), Univ. Duisburg, Germany, 387–389 (1987) (Experimental, 2)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
25
26
3 [1987Kis]
[1987Lev]
[1987Pyz] [1987Sar]
[1988Kov]
[1989Blu]
[1989Hal] [1989Kha]
[1990Ase]
[1990Luk]
[1990Oka]
[1990Pyz]
[1990Ram] [1991Kha1]
[1991Kha2]
[1991Kha3]
[1991Kha4]
[1991Pri]
Al–B–C Kisly, P.S., Prikhna, T.A., Gontar A.N., Podarevskaya, O.V., “Structure and Properties of Monocrystals of the Al-B-C System Compounds” in “Boron, Borides and Related Compounds”, Proceedings 9th Int. Sympos., Werheit, H. (Ed), Univ. Duisburg, Germany, 273–274 (1987) (Thermodyn., Crys. Structure, Phys. Prop., Experimental, 1) Levinskas, D., “Evaluation of Boron Carbide Coatings”, Western Region American Nuclear Society Student Conference: Nuclear Technology for the Year 2000, American Nuclear Society, La Grange Park, IL., NM(USA), 68–71 (1987) (Experimental, 0) Pyzik, A.J., Aksay, I.A., “Multipurpose Boron Carbide-Aluminum Composite and its Manufacture via the Control of the Microstructure”, US patent document 4,702,7707 A/, 27, (1987) Sarikaya, M., Laoui, T., Milius D.L., Aksay, I.A., “Identification of a New Phase in the Al-B-C Ternary by High-Resolution Transmission Electron Microscopy”. Proc. 45th Ann. Meeting of the Electron Microscopy Society of America, Bailey, G.N., (Ed.), San Franc. Press, USA, 168–169 (1987) (Crys. Structure, Experimental, 4) Koval’chenko, M.S., Paustovskij, A.V., Bolejko, B.M. Zhidkov, A.V., “Laser Surface Hardening of Cermets on the Base of Boron Carbide”(in Russian), Poroshk. Metall., 5, 77–80 (1988) (Mechan. Prop., Experimental, 6) Blumenthal, W.R., Gray, G.T., “Structure-Property Characterization of Shock-Loaded B4C-Al”, Inst. Phys. Conf. Ser. No 102: Session 7, Paper Presented at Int. Conf. Mech. Prop. Materials at High Rates of Strain, Oxford, 363–370 (1989) (Experimental, 8) Halverson, D.C., Pyzik, A.J., Aksay, I.A., Snowden, W.E., “Processing of Boron Carbide-Aluminium Composites”, J. Am. Ceram. Soc., 72(5), 775–80 (1989) (Experimental, 33) Kharlamov, A.I., Duda, T.I., Lojchenko, S.V., Fomenko, V.V., “Preparation and Properties of Aluminium Boridocarbide Powder of Al8B4C7 Composition”, 12thUkrainian Republic Conference on Inorganic Chemistry, Vol. 1, Simferopol’, Ukr. SSR, 44pp. (1989) (Mechan. Prop., Experimental, 0) Aselage, T.L., Tallant, D.R., Gieske, J.H., “Preparation and Properties of Icosahedral Borides” in “The Physics and Chemistry of Carbides, Nitrides and Borides”, Freer, R. (Ed.), Proc. NATO Advanced Research Workshop, Manchester, U.K., 1989, published as ASI-Series, Ser. E: Appl. Sci., Vol. 185, Kluwer Acad. Publ., Dordrecht, 97–111 (1990) (Crys. Structure, Review, Experimental,14) Lukas, H.L., “Aluminium-Boron-Carbon” in “Ternary Alloys. A Comprehensive Compendium of Evaluated Constitutional Data and Phase Diagrams”, Petzow, G., Effenberg, G., (Eds.), Vol. 3, VCH, Weinheim, 140–146 (1990) (Review, Phase Diagram, 14) Okada, S., Kudou, K., Hiyoshi, H., Higashi, I., Hamano, K., Lundstro¨m, T., “Preparation of AlC4B24 and Al3C2B48 Crystals”, J. Int. Ceram. Soc. Jpn., 98, 1342–1347 (1991), translated from Nippon Seramikkusu Kyokai Gakujutsu Ronbunshi, 98(12), 1330–1336 (1990) (Experimental, Crys. Structure, 24) Pyzik, A.J., Williams P.D., McCombs, A., “New Low Temperature Processing for Boron Carbide/ Aluminium Based Composite Armor”, Final Report, US-Army Research Office, DAAL 0388 C0030, 1990 (Experimental, 14) Ramesh, K. T., Ravichandran, G., “Dynamic Behavior of a Boron Carbide-Aluminum Cermet: Experiments and Observations”, Mech. Mater., 10(1-2) 19–29 (1990) (Experimental, 22) Kharlamov, A.I., Loichenko, S.V., “Electronic Transport Properties of Hot-pressed Boron-rich Compounds of the Al-B-C System” in “Boron-Rich Solids”, AIP Conf. Proc. 231, Emin, D. et al (Eds.), Albuquerque, USA, 1990, AIP, New York, 94–97 (1991) (Experimental, 5) Kharlamov, A.I., Loichenko, S.V., “Investigation: The Process of Densification of Boron-Rich Compounds of the Al-B-C System” in “Boron-Rich Solids”, AIP Conf. Proc. 231, Emin, D. et al (Eds.), Albuquerque, USA, 1990, AIP, New York, 473–481 (1991) (Experimental, 2) Kharlamov, A.I., Murzin, L.M., Loichenko, S.V., Duda, T.I., “Electrical Conductivity and Seebeck Coefficient of Hot-Pressed Specimens of Aluminium Borides and Carboborides”, Sov. Powder Metall. Met. Ceram., 9(345), 770–773 (1991), translated from Poroshk. Metall., 9(345), 62–65 (1991) (Experimental, Electr. Prop., 7) Kharlamov, A.I., Duda, T.I., Fomenko, V.V., “Preparation and Properties of High-Dispersive Powders of Aluminium Dodecaboride and Carboborides” in “Boron-Rich Solids”, AIP Conf. Proc. 231, Emin, D. (Eds.), Albuquerque, USA, 1990, AIP, New York, 512–515 (1991) (Experimental, 0) Prikhina, T.A., Kisly, P.S., “Aluminium Borides and Carboborides” in “Boron-Rich Solids”, AIP Conf. Proc. 231, Emin, D. et al (Eds.), Albuquerque, USA, 1990, AIP, New York, 590–593 (1991) (Experimental, 11)
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C [1991Pyz] [1992Bei] [1992Var] [1992Via] [1993Bau]
[1993Gon]
[1993Ips] [1993Kau] [1993Wen] [1993Wer]
[1994Dus] [1994Kud]
[1995Bon] [1995Hil] [1995Osc] [1995Pyz]
[1995Rug] [1996Bid] [1996Hil1]
[1996Hil2]
[1996Kas] [1996Pyz] [1996RMi]
[1996Vin]
3
Pyzik, A.J., Nilson, R.T., “B4C/A1 Cermets and Method for Making Same”, US Patent Document 5,039,633, (1991) Beidler, C.J., Hauth III, W.E., Goel, A., “Development of a B4C/A1 Cermet for Use as an Improved Structural Neutron Absorber”, J. Testing and Evaluation, 20(1), 67–70 (1992) (Experimental, 6) Vardiman, R.G., “Microstructures in Aluminium, Ion Implanted with Boron and Heat Treated”, Acta Metall. Mater., 40, 1029–35 (1992) (Crys. Structure, Eperimental, 7) Viala, J.C., Gonzales, G., Bouix, J., “Composition and Lattice Parameters of a New Aluminium-Rich Boron Carbide”, J. Mater. Sci. Lett., 11, 711–714 (1992) (Crys. Structure, Experimental, 9) Bauer, J., Bittermann, H., Rogl, P., “Phase Relations and Structural Chemistry in the Ternary System Aluminium - Boron - Carbon”, COST-507, Annual Report, (1993) (Crys. Structure, Phase Diagram, Experimental, 12) Gonzalez, G., Esnouf, C., Viala, J.C., “Structural Study of a New Aluminium Rich Borocarbide Formed by Reaction at the B4C/Al Interface”, Mater. Sci. Forum, 126-128, 125–128 (1993) (Crys. Structure, Experimental, 4) Ipser, H., privat communication (1993) (Experimental) Kaufmann, L., private communication (1993) (Thermodyn.) Wen, H., “Thermodynamic Calculations and Constitution of the Al-B-C-N-Si-Ti System” (in German), Thesis, Univ. Stuttgart, 1–183 (1993) (Calculation, Phase Diagram, Thermodyn., 223) Werheit, H., Kuhlmann, U., Laux, M., Lundstro¨m, T., “Structural and Electronic Properties of CarbonDoped β-Rhombohedral Boron”, Phys. Status Solidi (B), B179, 489–511 (1993) (Crys. Structure, Experimental, 51) Duschanek, H., Rogl, P., “The System Al-B”, J. Phase Equilib., 15(5), 543–52 (1994) (Crys. Structure, Phase Diagram, Experimental, #, 78) see also ibid, 16(1), 6 (1995) Kudou, K., Okada, S., Hikichi, H., Lundstro¨m, T., “Preparation and Properties of Si-doped Al3C2B48Type Crystals” (in Japanese), J. Soc. Mater. Sci., Jpn., 43(485), 223–228 (1994) (Experimental, Crys. Structure, Phys. Prop., 20) Bond, G.M., Inal, O.T., “Shock-Compacted Aluminium/Boron Carbide Composites”, Compos. Eng. 5(1), 9–16 (1995) (Experimental, 18) Hillebrecht, H., Meyer, F., “B48A13C2 - a Filled Variant of Tetragonal Boron”, Z. Kristallogr., Suppl. 10, 101 (1995) (Crys. Structure, Experimental, 2) Oscroft, R.J., Roebuck P.H.A., Thompson, D.P., “Characterisation and Range of Composition for Al8B4C7”, Br. Ceram. Trans., 94(1), 25–26 (1995) (Experimental, 11) Pyzik, A.J., Beaman, D.R., “Al-B-C Phase Development and Effects on Mechanical Properties of B4C/ Al-Derived Composites”, J. Am. Ceram. Soc., 78(2), 305–312 (1995) (Crys. Structure, Mechan. Prop., Experimental, 25) Ruginets, R., Fischer, R. “Microwave Sintering of Boron Carbide Composites”, Am. Ceram. Soc. Bull., 74(1), 56–58 (1995) (Experimental) Bidaud, E., research at Univ. Wien, unpublished (1996) Hillebrecht, H., Meyer, F.D., “The Structure of B48Al3C2 - A Filled and Distorted Variant of Tetragonal Boron (I)” in “Boron, Borides and Related Compounds”, Proc. 12th Int. Symp., Baden/Wien, paper PA.4, 59 (1996) (Crys. Structure, Experimental, 6) Hillebrecht, H., Meyer, FD., “Synthesis, Crystal Structure, and Vibrational Spectra of Al3BC3, a Carbidecarboborate of Aluminium with Linear (C=B=C)5– Anions”, Angew. Chem., 35(21), 2499–2500 (1996), translated from Angew. Chemie, 108(21), 2655–2657 (1996) (Crys. Structure, Experimental, 17) Kasper, B., “Phase Equilibria in the B-C-N-Si System”, Thesis, Max Plank Institute-PML, Stuttgart, (1996) (Phase Diagram, Thermodyn.) Pyzik, A.J., Deshmukh, U.V., Dunmead, S.D., Ott, J.J., Allen, T.L., Rossow, H.E., “Light Weight Boron Carbide/Aluminium Cerments”, United States Patent: 5,521,016, (1996) R’Mili, M., Massardier, V., Merle, P., Vincent, H., Vincent, C., “Mechanical Properties of T300/A1 Composites. Embrittlement Effects due to a B4C Coating”, J. Mater. Sci., 31, 4533–4539 (1996) (Mechan. Prop., Experimental, 12) Vincent, H., Vincent, C., Berthet, M. P., Bouix, J., Gonzalez, G., “Boron Carbide Formation from BCl3CH4-H2 Mixtures on Carbon Substrates and in a Carbon-Fibre Reinforced Al Composite”, Carbon, 34 (9), 1041–1055 (1996) (Crys. Structure, Mechan. Prop., Experimental, 25)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
27
28
3 [1997Du] [1997Mey] [1997Sch]
[1997Via] [1997Yue] [1998Kas]
[1998Kha]
[1998Rog]
[1999Bur] [1999Cha]
[1999Tor]
[1999Tsu] [2000Hal]
[2000Hig] [2000Kha]
[2000Liu] [2000Mey]
[2000Pyz] [2000Sav] [2000Sol] [2000Wan]
Al–B–C Du, W.F., Watanabe, T., “High-Toughness B4C-AlB12 Composites Prepared by Al Infiltration”, J. Eur. Ceram. Soc., 17, 879–884 (1997) (Mechan. Prop., Experimental, 15) Meyer, F.D. Hillebrecht, H., “Synthesis and Crystal Structure of Al3BC, the First Boridecarbide of Aluminium”, J. Alloy. Compd., 252, 98–102 (1997) (Crys. Structure, Experimental, 30) Schmechel, R., Werheit, H., Robberding, K., Lundstro¨m, T., Bolmgren, H., “IR-active Phonon Spectra of B-C-Al Compounds with Boron Carbide Structure”, J. Solid State Chem., 133, 254–259 (1997) (Experimental, 11) Viala, J.C., Bouix, J., Gonzalez, G., Esnouf, C. “Chemical Reactivity of Aluminium with Boron Carbide”, J. Mater. Sci, 32, 4559–4573 (1997) (Phase Diagram, Experimental, 39) Yu¨cel, O., Tekin, A., “The Fabrication of Boron-Carbide-Aluminium Composites by Explosive Consolidation”, Ceram. Int., 23, 149–152 (1997) (Experimental, Mechan. Prop., 3) Kasper, B., Lukas, H.L., “System B-C” in “COST 507. Thermochemical Database for Light Metal Alloys”, Ansara, I., Dinsdale, A.T., Rand, M.H. (Eds.), Office for Official Publications of the European Communities, Belgium, Vol. 2, 117–119 (1998) (Review, Crys. Structure, Phase Diagram, Phase Relations, Thermodyn., 0) Kharlamov, A.I., Kirillova, N.V., Loichenko, S.V., Fomenko, V.V., “Properties of Aluminium Borides and Borocarbides”, Russ. J. Appl. Chem., 71(5), 743–749 (1998), translated from Zh. Prikl. Khim, 71(5), 717–724 (1998) (in Russian), (Crys. Structure, Kinetics, Mechan. Prop., Experimental, 13) Rogl, P., “Al-B-C (Aluminium-Boron-Carbon)”, MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.12170.2.20, (1998) aslo published in “Phase Diagrams of Ternary Metal-Boron-Carbon Systems”, Effenberg, G., (Ed.), ASM-Intl, MSI, 3–15 (1998) (Assessment, Crys. Structure, Experimental, Phase Diagram, 50) Burkhardt, U., Grin, Y., “Refinement of the Aluminium Diboride Crystal Structure” in “Borides and Related Compounds”, Abst. 13th Int. Symp. on Boron, Dinar (France), 13pp., (1999) (Crys. Structure, 3) Chapman, T.R., Niesz, D.E., Fox, R.T., Fawcett, T., “Wear-resistant Aluminum - Boron - Carbide Cermets for Automotive Brake Applications”, Wear, 236, 81–87 (1999) (Mechan. Prop., Experimental, 9) Torquato, S., Yeong, C.L.Y., Rintoul, M.D., Milius, D.L., Aksay, I.A., “Elastic Properties and Structure of Interpenetrating Boron Carbide/Aluminum Multiphase Composites”, J. Am. Ceram. Soc., 82(5), 1263–1268 (1999) (Mechan. Prop., 32) Tsuchida, T., Kan, T., “Synthesis of Al3BC in Air from Mechanically Activated Al/B/C Powder Mixtures”, J. Eur. Ceram. Soc., 19, 1795–1799 (1999) (Crys. Structure, Experimental, 12) Hall, A., Economy, J., “The Al(L)+AlB12ÐAlB2 Peritectic Transformation and its Role in the Formation of High Aspect Ratio AlB2 Flakes”, J. Phase Equilib., 21(1), 63–69 (2000) (Phase Diagram, Experimental, 21) Higashi, I., “Crystal Chemistry of α-AlB12 and γ-AlB12”, J. Solid State Chem., 154, 168–176 (2000) (Crys. Structure, Experimental, 18) Kharlamov, A. I., Nizhenko, V.I., Kirillova, N.V., Floka, L.I., “Wettability of Hot-Pressed Samples of Boron-Containing Aluminium Compounds by Liquid Metals and Alloys” (in Russian), Zh. Prikl. Khim., 73(6), 884–888 (2000) (Experimental, 14) Liu, C.H., “Structure and Properties of Boron Carbide with Aluminum Incorporation”, Mater. Sci. Eng. B, B72, 23–26 (2000) (Phys. Prop., Crys. Structure, Experimental, 10) Meyer, F.D., Hillebrecht, H., “Ternary Phases in the System Al/B/C” in “High Temperature Materials Chemistry”, Vol. 15, Part 1, K. Hilpert et al. (Eds.), Proc. 10th Intl. IUPAC Conf., Forschungszentrum Ju¨lich, Germany, Published by Schriften des Forschungszentrums Juelich, 161–164 (2000) (Crys. Structure, 5) Pyzik, A.J., Deshmukh, U.V., Krystosek, R. D., “Aluminum-Boron-Carbon Abrasive Article and Method to Form Said Article”, US Patent: 6,042,627, (2000). Savyak, M., Uvarova, I., Timofeeva, I., Isayeva L., Kirilenko, S., “Mechanochemical Synthesis in Ti-C, Ti-B, B-C, B-C-A1 Systems”, Mater. Sci. Forum, 343-346, 411–416 (2000) (Experimental, 4) Solozhenko, V.L., Meyer, F.D., Hillebrecht, H., “300-K Equation of State and High-Pressure Phase Stability of Al3BC3”, J. Solid State Chem., 154, 254–256 (2000) (Crys. Structure, Experimental, 11) Wang, T., Yamaguchi, A., “Some Properties of Sintered Al8B4C7”, J. Mater. Sci. Letter., 19, 1045–1046 (2000) (Calculation, Crys. Structure, 6)
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–C [2000Wer] [2001Fje]
[2001Lee]
[2002Ars] [2002Bur]
[2002Kou1] [2002Kou2]
[2002Zhe] [2003Per]
[Mas2] [V-C2]
3
Werheit, H., Schmechel, R., Meyer, F.D., Hillebrecht, H., “Interband Transitions and Optical Phonons of B48Al3C2”, J. Solid State Chem., 154, 75–78 (2000) (Optical Prop., Experimental, 10) Fjellstedt, J., Jarfors, A.E.W., El-Benawy, T., “Experimental Investigation and Thermodynamic Assessment of the Al-rich Side of the Al-B System”, Mater. Des., 22(6), 443–449 (2001) (Thermodyn, Phase Diagram, Experimental, 14) Lee, K.B., Sim, H.S., Cho, S.Y., Kwon, H., “Reaction Products of Al-Mg/B4C Composite Fabricated by Pressureless Infiltration Technique”, Mater. Sci. Eng. A, 302, 227–234 (2001) (Crys. Structure, Phase Diagram, Experimental, 17) Arslan, G., Kara, F., Turan, S., “Mechanical Properties of Melt Infiltrated Boron Carbide-Aluminium Composites”, Key Eng. Mater., 206-213(2), 1157–1160 (2002) (Experimental, Mechan. Prop., 5) Burkhardt, U., Gurin, V., Borrmann, H., Schnelle, W., Grin, Y., “On the Electronic and Structural Properties of Aluminium Diboride Al0.9B2” in “Boron, Borides and Related Compound”, Abst. 14th Int. Symp., (ISBB’02), Saint Petersburg, O4, (2002) (Crys. Structure, 3) Kouzeli, M., Mortensen, A., “Size Dependent Strengthening in Particle Reinforced Aluminium”, Acta Mater., 50, 39–51 (2002) (Mechan. Prop., Experimental, 59) Kouzeli, M., Marchi, C. S., Mortensen, A., “Effect of Reaction on the Tensile Behavior of Infiltrated Boron Carbide-Aluminum Composites”, Mater. Sci. Eng. A, A337, 264–273 (2002) (Experimental, Mechan. Prop., 51) Zheltov, P., Grytsiv, A., Rogl, P., Velikanova, T.Ya., Research at Univ. Wien (unpublished) (2002) (Phase Diagram, Crys. Structure) Perrot, P., “Aluminium-Carbon”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart, to be published, (2003) (Phase Diagram, Crys. Structure, Assessment, 19) Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_3 ß Springer 2009
29
Al–B–Mo
4
Aluminium – Boron – Molybdenum Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Qingsheng Ran, updated by Lazar Rokhlin, Tatiana Dobatkina, Elena Semenova, Natalia Kol’chugina
Introduction The Al-B-Mo system is of interest mainly because of the application of low-alloyed Mo compositions in manufacturing parts for operation under conditions of high-temperature gases and erosion wear [1988Buk, 1994Buk, 1995Buk, 1997Buk, 1999Buk, 2003Buk1, 2003Buk2]. The first evaluation within the ongoing MSIT Evaluation Program was made by [1990Ran], which is updated by the present work. An isothermal section at 1000˚C was presented by [1965Rie] obviously from the determination of phase regions using X-ray diffraction. Metals were cold pressed; samples were prepared by reacting at 900˚C and annealing at 1200˚C for 15 h. While cooling, equilibrium was said to be frozen in at 1000˚C. [1942Hal] prepared a ternary compound “Mo7Al6B7” by thermal reaction of MoO3, B2O3, Al and S and attempted a first indexation of its powder pattern. The existence of the phase was later confirmed by [1965Rie, 1966Jei], which assumed that its formula is MoAlB. Moreover, an Al-stabilized molybdenum boride with the CrB type structure was found. To investigate the structure of this phase more accurately, [1966Jei] heated a sample of the composition Mo:Al:B = 1:6:1 to about 1800˚C and cooled it for 40 minutes to 1000˚C. The charge was subsequently treated in hot NaOH solution and single crystals were obtained from the residue. In performing X-ray diffraction, the Debye-Scherrer, Weissenberg, and rotating crystal methods were used. In [1977Gur], crystals of solid solutions of boron (to 1 mass%) in MoAl4(5) were separated from Al-B-Mo alloys (the alloys were prepared preliminarily by melting followed by spontaneous solidification) by dissolution of Al matrix in HCl. The MoAlB (orthorhombic) compound and another compound of the Al-B-Mo system with a rhombohedral crystal structure were reported by [1976Hig]. Reviews [1972Cha, 1976Hig] included the aforementioned data on the phases existing in the ternary Al-B-Mo system. Investigations into the Al-B-Mo phase relations, structure identifications are given in Table 1.
Binary Systems The binary systems Al-B [2004Mir] (Fig. 1), B-Mo [1992Rog] (Fig. 2), and Al-Mo [2005Sch] are accepted in the present assessment. Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
1
2
4
Al–B–Mo
Solid Phases The solid phases of the Al-B-Mo system are described in Table 2 that is presented mainly with allowance for the binary phase diagrams accepted in this assessment. Two ternary phases were found in the system; these are τ1 (MoAlB) and τ2 (Mo9AlB10). The homogeneity ranges of the phases are taken from the isothermal section at 1000˚C given by [1965Rie]. The aluminium solubility in B-Mo phases and boron solubility in Al-Mo phases are taken also from this section. Virtually the same boron solubility in MoAl4 was confirmed by [1977Gur].
Isothermal Sections The only isothermal section at 1000˚C (Fig. 3) is constructed based on data by [1965Rie] corrected with allowance for the binary phase diagrams accepted in the present evaluation. In accordance with the binary B-Mo system, the existing MoB4 compound is added in Fig. 3; two three-phase regions containing the MoB4 phase in the section are given tentatively. The MoAl4 and Mo4Al17 compounds are added to the section after the accepted binary Al-Mo system. They are located between the Al rich liquid and Mo3Al8 that are in equilibrium with the τ1 phase. Therefore, it was reasonable to accept the existence of the MoAl4 and Mo4Al17 compounds in equilibrium with the τ1 phase. This is indicated in the section in Fig. 3.
Notes on Materials Properties and Applications Owing to the importance of molybdenum-based alloys containing small amounts of Al and B for the manufacturing of parts for operation under conditions of high-temperature gases and erosion wear, various mechanical properties of them have been investigated at room and high temperatures [1988Buk, 1994Buk, 1995Buk, 1997Buk, 1999Buk, 2000Buk, 2003Buk1, 2003Buk2]. Table 3 shows the mechanical properties and their correlation with the structural state.
Miscellaneous The possibility of forming composites with Al matrix strengthened by molybdenum borides is considered in [1996Bie].
. Table 1 Investigations of the Al-B-Mo Phase Relations, Structures and Thermodynamics Reference [1942Hal]
Method/Experimental Technique
Temperature/Composition/Phase Range Studied
Interaction of molybdenum boride with 74 mass% Mo, 18 mass% Al, 8.5 aluminium followed by dissolution of Al mass% B / near Mo7Al6B7 matrix / X-ray diffraction, chemical analysis, density measurements
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Mo
4
. Table 1 (continued) Reference
Method/Experimental Technique
Temperature/Composition/Phase Range Studied 1000˚C / 0–80 at.% Al, 0–100 at.% Mo, 0–100 at.% B /
[1965Rie]
Cold pressing of powders followed by heating, X-ray diffraction
[1966Jei]
Heating of components to 1800˚C followed 1000˚C / MoAlB by slow cooling, chemical extraction / X-ray diffraction
[1977Gur] Melting followed by chemical extraction after solidification / X-ray diffraction, chemical analysis
1400–1000˚ / 55 mass% Al, 43 mass% Mo, 0.7 mass% B / MoAl4-based solid solution of B
. Table 2 Crystallographic Data of Solid Phases
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
(βAl)
hP2 P63/mmc Mg
a = 269.3 c = 439.8
at 25˚C, 20.5 GPa [Mas2]
(αAl) < 660.452
cF4 Fm 3m Cu
a = 404.96
at 25˚C [Mas2]
(βB) < 2092
hR333 R3m βB
a = 1093.30 c = 2382.52
[1993Wer]
a = 1093.02 c = 2381.66
pure B [1976Lun]
a = 1006.1 c = 1421.0
presumably metastable phase, possibly stabilized by impurities, preparation at 1100 to 1400˚C [1971Amb]
(B) (tetr.)
tP192 derived from αAlB12
(αB)
hR36 R 3m αB
(Mo) < 2623
Landolt‐Bo¨rnstein New Series IV/11E1
cI2 Im 3m W
a = 490.8 c = 1256.7 a = 314.70
MSIT1
presumably metastable phase, preparation below 1000˚C [1971Amb] pure B, single crystal [1994Cha] at 25˚C [Mas2] dissolves up to 19.5 at.% Al and up to 1 at.% B [2005Sch, Mas2]
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
3
4
4
Al–B–Mo
. Table 2 (continued)
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
αAlB12 < 2094
oP384 P212121 αAlB12
a = 1662.3 b = 1754.0 c = 1018.0
[2004Mir] [V-C2]
γAlB12 ≤ 1550
oP396 P212121 γAlB12
a = 1662.3 b = 1754.0 c = 1018.0
[1983Hig] Metastable or metal impurity stabilized [1994Dus]
AlB2 < 972 - 213
hP3 P6/mmm AlB2
a = 300.5 c = 325.7
[2004Mir] [V-C2]
MoAl12 < 712
cI26 Im 3 WAl12
a = 757.3
[2005Sch] 92.3 at.% Al
MoAl5(h2) 846 - (750 - 800)
hP12 P6322 WAl5
a = 491.2
[2005Sch] 83.3 at.% Al
a = 493.3 c = 4398
[2005Sch] 83.3 at.% Al
MoAl5(h1) hP60 (750–800) - 648 P321 MoAl5(h1) MoAl5(r) ≲ 648
hP36 R 3c MoAl5(r)
a = 495.1 c = 2623
[2005Sch] 83.3 at.% Al
Mo5Al22(h) 964 - 831
oF216 Fdd2 Mo5Al22(h)
a = 7382 ± 3
[2005Sch] 81.5 at.% Al
Mo4Al17 < 1034
mC84 C2 Mo4Al17
a = 915.8 ± 0.1 b = 493.23 ± 0.08 c = 2893.5 ± 0.5 β = 96.71 ± 0.01˚
[2005Sch] 81 at.% Al
MoAl4(h) 1177 - 942
mC30 Cm WAl4
a = 525.5 ± 0.5 [2005Sch] b = 1776.8 ± 0.5 79 at.% Al c = 522.5 ± 0.5 β = 100.88 ± 0.06˚
Mo1–xAl3+x 1260 - 1154
cP8 Pm 3n Cr3Si
a = 494.5 ± 0.1
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
MSIT1
[2005Sch] 76.5 at.% Al
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Mo
4
. Table 2 (continued)
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
MoAl3(h) 1222 - 818
mC32 C2/m MoAl3
a = 1639 ± 1.0 [2005Sch] b = 359.4 ± 0.1 75 at.% Al c = 838.6 ± 0.4 β = 101.88 ± 0.07˚
Mo3Al8 < 1555 ± 10
mC22 Cm Mo3Al8
a = 920.8 ± 0.3 [2005Sch] b = 363.78 ± 0.03 72.7 at.% Al c = 1006.5 ± 0.3 β = 100.78 ± 0.05˚
ζ1(h), Mo2Al3(h) 1570 - 1490
Unknown
-
[2005Sch] 63 at.% Al
ζ2(h), MoAl(h) 1750 - 1535
cP2 Pm 3m CsCl
a = 309.8
[2005Sch] 50–52 at.% Al
Mo3Al ≲ 2150
cP8 Pm 3n Cr3Si
a = 495.0
[2005Sch] 23–29 at.% Al
Mo2B < 2280
tI12 I4/mcm Al2Cu
a = 554.7 c = 473.9
[Mas2] [V-C2] 33 at.% B
αMoB < 2180
tI16 I41/amd MoB
a = 310.3 c = 1695
[Mas2] [V-C2] 48–50 at.% B
βMoB 2600 - 2180
oC8 Cmcm CrB
MoB2 2375 - 1517
hP3 P6/mmm AlB2
a = 303.9 c = 305.5
[Mas2] [V-C2] 62–66 at.% B
Mo2B5 < 2140
hR21 R3m Mo2B5
a = 300.7 c = 2091.0
[Mas2] [V-C2] 67–69 at.% B
MoB4 < 1807
hP20 P63/mmc WB4
a = 520.3 c = 634.5
[Mas2] [V-C2] 79 at.% B
Landolt‐Bo¨rnstein New Series IV/11E1
a = 315.1 b = 847.0 c = 308.2
MSIT1
[Mas2] [V-C2] 48–51 at.% B
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
5
6
4
Al–B–Mo
. Table 2 (continued)
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
* τ1, MoAlB ≲ 1000˚C
oC12 Cmcm BCU
a = 321.2 b = 1398.5 c = 310.2
[1966Jei, V-C2] 31–34.5 at.% B and 33–35.5 at.% Al
* τ2, Mo9AlB10
oC8 Cmcm CrB
a = 316.3 b = 847.5 c = 308.2
[V-C2] 48–50 at.% B and 5–6.5 at.% Al
. Table 3 Investigations of the Al-B-Mo Materials Properties Reference
Method / Experimental Technique
Type of Property
[1988Buk]
Tensile creep tests at 1500–2000˚C. Creep rate and stress-rupture strength for Mobased compositions low-alloyed with Al and B
[1994Buk]
Tensile creep tests 1500–2000˚C.
Correlation between short-term, long-term, and low-cycle strength characteristics of Mo-based compositions low-alloyed with Al and B were established.
[1995Buk]
Tensile tests 20–2000˚C.
Ultimate strength and relative elongation of Mo-based compositions low-alloyed with Al and B are determined.
[1997Buk]
Fatigue tests under conditions of rigid alternating bending at 950–1550˚C.
Effect of heat treatment and welding on fatigue resistance of Mo-based compositions lowalloyed with Al and B is studied.
[1999Buk]
Tensile tests at (0.5–0.8) Tm.
Correlation between short-term, long-term static, creep resistance, and few-cycle strength characteristics of Mo-based compositions lowalloyed with Al and B were established.
[2000Buk]
Tensile and fatigue tests under conditions of rigid alternating bending.
Empirical correlations between fatigue strength, conventional yield strength, and grain size were established.
[2003Buk1] Tensile tests at 20–2000˚C and fatigue tests.
Correlations between the structural state and short-term and low- and high-cycle fatigue were established.
[2003Buk2] Tensile tests at 20–2000˚C.
Effect of heat treatment on ultimate strength, yield strength, relative elongation, and relative uniform deformation is considered.
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Mo
4
. Fig. 1 Al-B-Mo. The Al-B binary system
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
7
8
4
Al–B–Mo
. Fig. 2 Al-B-Mo. The B-Mo binary system
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Mo
4
. Fig. 3 Al-B-Mo. Isothermal section at 1000˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
9
10
4
Al–B–Mo
References [1942Hal] [1965Rie]
[1966Jei] [1971Amb] [1972Cha]
[1976Hig] [1976Lun] [1977Gur]
[1983Hig] [1988Buk]
[1990Ran]
[1992Rog]
[1993Wer]
[1994Buk]
[1994Cha]
[1994Dus] [1995Buk]
[1996Bie]
Halla, F., Thury, W., “On Borides of Molybdenum and Tungsten” (in German), Z. Anorg. Allg. Chem., 249, 229–237 (1942) (Crystal Structure, Experimental, 7) Rieger, W., Nowotny, H., Benesovksy, F., “Complex Borides of the Transition Metals (Mo, W, Fe, Co, Ni)” (in German), Monatsh. Chem., 96(3), 844–851 (1965) (Crys. Structure, Experimental, Phase Diagram, #, 10) Jeitschko, W., “The Crystal Structure of MoAlB” (in German), Monatsh. Chem., 97, 1472–1476 (1966) (Crys. Structure, Experimental, 10) Amberger, E., Ploog, G., “Formation of Lattices of Pure Boron” (in German), J. Less-Common Met., 23, 21–31, (1971) (Crys. Structure, Experimental, 17) Chaban, N.F., Kuz’ma, Yu.B., “Metallides in the Period IV Transition Metal-Aluminum (Gallium) Boron Ternary System” (in Russian), Stroenie, Svoistva i Primenenie Metall., 102–107 (1972) (Crys. Structure, Experimental, Phase Diagram, Phase Relations, Review, 18) Higashi, I., Takahashi, Y., Atoda, T., “Crystal Growth of Borides and Carbides of Transition Metals from Al Solutions”, J. Cryst. Growth, 33, 207–211 (1976) (Experimental, 16) Lundstro¨m, T., Tergenius, L.E., “On the Solid Solution of Copper in β-Rhombohedral Boron”, J. LessCommon Met., 47, 23–28 (1976) (Crys. Structure, Experimental, 10) Gurin, V.N., Korsukova, M.M., Popov, V.I., Elizarova, O.V., Belozov, N.N., Kuz’ma, Yu.B., “Solid Solutions of B, C, Si in Aliminides of Transient Metals” (in Russian), Akad. Nauk SSSR, Nauka, Moscow, 39–42 (1977) (Crys. Structure, Experimental, Phase Diagram, 6) Higashi, I., “Aluminum Distribution in the Boron Framework of γ-AlB12”, J. Solid State Chem., 47, 333–349 (1983) (Experimental, Crys. Structure, 21) Bukhanovskii, V.V., Kharchenko, V.K., Polishchuk, E.P., Kravchenko, V.S., Galinzovskaya, T.D., Onoprienko, A.A., “Influence of Production Factors on the High-Temperature Strength Characteristics of Molybdenum Alloys”, Strength Met., 20(6), 818–824 (1988), translated from Probl. Prochn., (6), 102–108 (1988) (Experimental, Kinetics, Morphology, 18) Ran, Q., “Al-B-Mo (Aluminium-Boron-Molybdenum)” in MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.19496.1.20, (1990), also published in “Ternary Alloys”, Petzow, G., Effenberg, G. (Eds.), Vol. 3, VCH Verlagsgesellschaft, Weinheim, Germany, 189–191 (1990) (Phase Diagram, Phase Relations, Review, 5) Rogl, P., “The system B-N-Mo” in “Phase Diagrams of Ternary Boron Nitride and Silicon Nitride Systems”, Rogl, P., Schuster, J. (Eds.), Ohio, USA: ASM, Materials Park, 64–67 (1992) (Crys. Structure, Phase Diagram, Phase Relations, Thermodyn., Experimental, Review, *, 10) Werheit, H., Kuhlmann, U., Laux, M., Lundstro¨m, T., “Structural and Electronic Properties of CarbonDoped β-Rhombohedral Boron”, Phys. Stat. Sol. B, 179(2), 489–511 (1993) (Crys. Structure, Experimental, 51) Bukhanovskii, V.V., Borisenko, V.A., Kharchenko, V.K., “Correlations Between Short-Term, Long-Term Static, and Low-Cycle Strength Characteristics of Low-Alloy Molybdenum Alloys at High Temperatures”, Strength Met., 28(12), 895–902 (1994), translated from Probl. Prochn., (12), 43–51 (1994) (Experimental, Mechan. Prop., 21) Chakrabarti, D.J., Laughlin, D.E., “B-Cu (Boron-Copper)” in “Phase Diagrams of Binary Copper Alloys”, Subramanian, P.R., Chakrabarti, D.J., Laughlin, D.E. (Eds.), ASM International, Materials Park, OH, 74–78 (1994) (Review, Phase Diagram, Crys. Structure, Thermodyn., 24) Duschanek, H., Rogl, P., “The Al-B (Aluminum-Boron) System”, J. Phase Equilib., 15, 543–552 (1994) (Assessment, Crys. Structure, Phase Relations, Phase Diagram, Review, Thermodyn., 78) Bukhanovskii, V.V., Borisenko, V.A., Kharchenko, V.K., “Mechanical Characteristics of Molybdenum Alloys of the Systems the Mo-Al-B and Mo-Zr-B in the Temperature Range 290–2270 K”, Strength Met., 27(11-12), 688–695 (1995), translated from Probl. Prochn., 27(11-12), 70–80 (1995) (Experimental, Mechan. Prop., 19) de Bie, J.E., Froyen, L., Lust, P., Delaey, L., “Solidification of In-Situ Aluminium Composites”, Mater. Sci. Forum, 215-216, 435–442 (1996) (Morphology, Phase Relations, Theory, 10)
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Mo [1997Buk]
[1999Buk] [2000Buk]
[2003Buk1]
[2003Buk2]
[2004Mir]
[2005Sch]
[Mas2] [V-C2]
4
Bukhanovskii, V.V., Borisenko, V.A., Kharchenko, V.K., “Effect of Heat Treatment and Welding on the Fatigue Resistances of Molybdenum Alloys of the Mo-Zr-B and Mo-Al-B Systems”, Met. Sci. Heat Treat., 39(5-6), 247–250 (1997), translated from Metalloved. Term.. Obrab. Met., (6), 16–19 (1997) (Experimental, Mechan. Prop., 8) Bukhanovskii, V.V., “Correlation Between the Strength and Creep of Molybdenum and Tungsten Alloys”, Russ. Metall. (Engl. Transl.), (5), 91–98 (1999) (Experimental, Mechan. Prop., 22) Bukhanovskii, V.V., “Correlations between the Characteristics of Fatigue Resistance, Short-Term Strength, and Structure of Low-Molybdenum Alloys”, Strength Met., 32(4), 361–367 (2000), translated from Probl. Prochn., (4), 75–85 (2000) (Experimental, Mechan. Prop., 14) Bukhanovsky, V., Mamuzic, I., Borisenko, V., “Interrelation between the Structural State of Material and Mechanical Properties of Low-Alloyed Molybdenum Alloys”, Metallurgia, 42(3), 159–166 (2003) (Experimental, Kinetics, Mechan. Prop., 25) Bukhanovsky, V.V., Mamuzic, I., Borisenko, V.A., “The Effect of Thermal Treatment on the Mechanical Properties of Low-Alloyed Molybdenum Alloys Over the Wide Range of Temperatures”, Metallurgia, 42(1), 9–14 (2003) (Experimental, Morphology, Mechan. Prop., 20) Mirkpvic, D., Gro¨bner, J., Schmid-Fetzer, R., Fabrichnaya, O., Lukas, H.L., “Experimental Study and Thermodynamic Re-Assessment of the Al-B System,” J. Alloys Compd., 384, 168–174 (2004) (Phase Diagram, Phase Relations, Thermodyn., Assessment, Calculation, #, 26) Schuster, J.C., “Al-Mo (Aluminum-Molybdenum)”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services, GmbH, Stuttgart; Document ID: 30.12123.1.20, (2005) (Crys. Structure, Phase Diagram, Assessment, 61) Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_4 ß Springer 2009
11
Al–B–Si
5
Aluminium – Boron – Silicon Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Hans Leo Lukas
Introduction The first evaluation within the ongoing MSIT Evaluation Program was made by [1990Luk], which is updated by the present work. The only experimental ternary information on this system is the existence of a ternary phase Al3SiB48 [1969Lam, 1972Lam] (Table 1). There is evidence that this is a high temperature phase, which is easily quenchable to room temperature by rapid or moderate cooling. The previously reported βAlB12 phase is assumed to be identical with this phase, the structure of which is closely related to that of pure B. A phase with the same structure also appears as Al3B48C2 [1964Mat]. [1981Por] estimated interaction parameters of B and Si in the (Al) solid solution. [1982Doe] calculated the whole ternary phase diagram based on assessments of the binary subsystems. Since that time newer assessments for all three binary systems are available. Especially for the Al-B system good calorimetrically measured enthalpy data are available for the intermediate phases [2001Mes] increasing the quality of the new assessment of [2004Mir]. The diagrams given here are from calculations using the dataset of [2005Gro], which is composed of the binary assessments of Al-B [2004Mir], Al-Si [1996Gro] and B-Si [1998Fri]. They differ markedly from those of [1982Doe] although the reason is only a slightly more negative Gibbs energy of mixtures of the same overall compositions of AlB12 + Si compared to those of liquid-Al + B-Si phases, whereas in the dataset of [1982Doe] the contrary was assumed. The tie-lines between AlB12 and Si-Al melt, as calculated by [2005Gro], agree with experimental findings of [2005Yos1] [1999Wan, 2000Wan, 2003Nog, 2005Hui] investigated the influence of B-additions in the magnitude of 100 to 1000 mass-ppm to the morphology of the eutectic microstructure of hypoeutectic Al-Si alloys. The two newest ones did not find significant effects of B.
Binary Systems For the thermodynamic calculations the following assessments were merged by [2005Gro] to a ternary dataset: Al-B [2004Mir], Al-Si [1996Gro] and B-Si [1998Fri]. The phase diagrams calculated from these binary datasets agree well with those compiled in [Mas2], except Al-B, where [Mas2] assumes an additional phase AlB10, which was proved to be stable only as carbon containing ternary phase [1964Mat, 1994Dus].
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
1
2
5
Al–B–Si
Solid Phases One ternary phase, Al3SiB48, was reported by [1969Lam]. The authors got either this phase or αAlB12 on heating samples between 1400 and 1600˚C, indicating the upper temperature limit to be in this range. This phase was formerly described as binary phase βAlB12, however, [1964Mat] proved, that it is stable only with ternary additions, and gave a formula Al3B48C2. [1969Lam] showed, that carbon can be replaced in this phase by silicon, but not by germanium. The only stable binary Al-B phases are AlB2 and αAlB12 [1964Mat, 1994Dus]. Three more stable binary intermediate phases exist in the B-Si system, see Table 2. The crystal structures of the unary phases of pure boron are differently described in literature [V-C2]. The most likely interpretation is the existence of a phase hR36 below ca. 1100˚C and a high temperature phase B described by the Pearson symbols hR105, hR111 or hR141 regarding the number of atomic positions per rhombohedral unit cell. The hexagonal lattice parameters agree fairly well, a = 1092–1096, b = 2381–2389 pm. Regarding the partial occupations of the different structure descriptions, the number of atoms per rhombohedral unit cell is nearly equal for the different descriptions, 105–107. All well characterized solid phases are summarized in Table 2. Some of the crystal structures contain sites occupied only partially, there two Pearson symbols are given, one counting the sites, the other one counting the atoms per unit cell.
Invariant Equilibria Figure 1 shows the reaction scheme derived from calculations using the dataset of [2005Gro]. The calculated temperatures and phase compositions are given in Table 3. The scheme and especially the temperatures have to be taken as tentative. The temperature limits of Al3SiB48 are not known, there is only evidence that it forms between 1400 and 1600˚C and that it transforms at lower temperatures to another phase for which no details are known. Phase Al3SiB48 (τ) was added to the dataset of [2005Gro] as stoichiometric phase with linearly temperature dependent Gibbs energy forming peritectoidally at 1500˚C and neglecting the possible transformation. Below 1500˚C this phase appears everywhere in equilibrium with the three phases AlB12, SiB36 and SiB6.
Liquidus, Solidus and Solvus Surfaces The liquidus surface resulting from the calculation is shown in Fig. 2. It is remarkably different from that calculated from the dataset of [1982Doe] due to a newer assessment of the Al-B system [2004Mir] based on precise calorimetric measurements of the enthalpies of the AlB intermediate phases [2001Mes]. The isotherms are less dependent on the thermodynamic quantities than the curves of double saturation and therefore they should be taken as reasonably well defined.
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Si
5
Isothermal Sections The calculated isothermal sections at 1300 and 500˚C are shown in Figs. 3 and 4 respectively.
Temperature – Composition Sections Figure 5 shows a partial calculated Temperature - Composition section at 0.1 at.% B. Note that here the field L+AlB2+AlB12 is so narrow, that it is degenerated to a single line.
Thermodynamics There are no experimental data on ternary thermodynamic quantities. Some binary data, however, are very important for ternary calculations: the calorimetrically measured enthalpies of formation of AlB2 and AlB12 [2001Mes] as well as the enthalpy change during the invariant reaction L + AlB12 Ð AlB2 [2004Mir] A thermodynamic dataset was assessed by [2005Gro] by merging the binary datasets of [2004Mir] (Al-B), [1996Gro] (Al-Si) and [1998Fri] (B-Si) without using ternary terms.
Notes on Materials Properties and Applications Wang et al. [1999Wan, 2000Wan] reported a good refining effect of B on hypoeutectic Al-Si alloys, but [2003Nog] and [2005Hui] could not find a significant effect of B on the microstructure of the eutectic in Al-Si alloys. [2005Yos2] demonstrated, that “temperature gradient zone melting” (TGZM) with a thin Al-Si-melt may help to remove B-impurities from semiconductor grade Si material.
. Table 1 Investigations of the Al-B-Si Phase Relations, Structures and Thermodynamics Reference
Method/Experimental Technique
Temperature/Composition/Phase Range Studied
[1969Lam], Single-crystal X-ray diffraction [1972Lam]
Identification of the ternary phase τ, Al3SiB48
[2005Yos1] Distribution coefficient of B between Al-Si melt and solid Si
1100–1300˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
3
4
5
Al–B–Si
. Table 2 Crystallographic Data of Solid Phases Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
(Al) < 660.452
cF4 Fm3m Cu
a = 404.96
pure Al at 25˚C [V-C2]
(βB)(h) < 2092
hR315(a,b)
a = 1096 c = 2389
hR333(a), hR315(b)
a = 1093 c = 2381 a = 1093 c = 2382
three different complete structure descriptions, cited including atomic positions by [V-C2]
hR423(a), hR321(b) R3m βB
Lattice Parameters [pm]
Comments/References
(αB)(r)
hR36(c) R3m αB
a = 491.1 c = 1257.3
[V-C2] presumably metastable phase
(Si) < 1414
cF8 Fd3m C diamond
a = 543.06
at 25˚C, [V-C2]
γAlB12
oP396(a), oP377(b) P212121 γAlB12
a = 1662.3 b = 1754.0 c = 1018.0
[1983Hig] Metastable or metal impurity stabilized [1994Dus]
αAlB12 ≲ 2094
tP216(a), tP189(b) P41212 or P43212 αAlB12
a = 1016.1 c = 1428.3
[1977Hig]
AlB2 972 - ~213
hP3(a), hP2.9(b) P6/mmm AlB2
a = 300.9 c = 326.2
[1964Mat]
SiB36 < 2137
hR339(a), hR314(b)
a = 1101 [V-C2] c = 2390 a = 1099 to 1113 93.3 to 97 at.% B [1984Ole] c = 2383 to 2400
SiB6 < 1850
oP340(a), oP314.5(b) a = 1439.7 b = 1831.8 Pnnm c = 991.1 B6Si
R3m B36Si
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
MSIT1
[V-C2]
Landolt‐Bo¨rnstein New Series IV/11E1
5
Al–B–Si
. Table 2 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
B3Si < 1270
hR45 R3m B4C
* τ, Al3SiB48
tP68(a), tP52(b) P42/nnm B25C ?
Lattice Parameters [pm]
Comments/References
a = 632 to 635 [1984Ole] c = 1269 to 1275
(c)
a = 891 c = 505
[1969Lam] metastable at room temperature? Pearson symbol (a) and prototype [V-C2]
Pearson symbol showing number of sites per unit cell (for hR hexagonal unit cells) Pearson symbol showing number of atoms per unit cell (for hR hexagonal unit cells) (c) Number of atoms in Pearson symbol is valid for hexagonal unit cell. (a)
(b)
. Table 3 Invariant Equilibria Composition (at.%) Reaction
T [˚C]
Type
Phase
L + (βB) Ð αAlB12 + SiB36
2013
U1
L
L + SiB36 Ð αAlB12 + SiB6
αAlB12 + SiB36 + SiB6 Ð τ
L + SiB6 Ð αAlB12 + (Si)
Landolt‐Bo¨rnstein New Series IV/11E1
1838
≈1500
1373
U2
P1
U3
MSIT1
Al
B
Si
2.6
91.2
6.2
(B)
0.0
97.9
2.1
αAlB12
7.7
92.3
0.0
SiB36
0.0
96.7
3.3
L
1.9
63.0
35.1
SiB36
0.0
94.1
5.9
αAlB12
7.7
92.3
0.0
SiB6
0.0
86.2
13.8
αAlB12
7.7
92.3
0.0
SiB36
0.0
94.1
5.9
SiB6
0.0
86.2
13.8
τ
5.8
92.3
1.9
L
2.7
8.2
89.1
SiB6
0.0
85.5
14.5
αAlB12
7.7
92.3
0.0
(Si)
0.0
1.0
99.0
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
5
6
5
Al–B–Si
. Table 3 (continued) Composition (at.%) Reaction
T [˚C]
Type
Phase
SiB6 + (Si) Ð SiB3, αAlB12
1270
D1
SiB6
L + αAlB12 Ð AlB2 + (Si)
677
U4
B
Si
0.0
85.5
14.5
(Si)
0.0
0.7
99.3
SiB3
0.0
73.8
26.2
αAlB12
7.7
92.3
0.0
81.4
0.1
18.5
L αAlB12
L Ð (Al) + (Si), AlB2
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
577
D2
MSIT1
Al
7.7
92.3
0.0
AlB2
33.3
66.7
0.0
(Si)
0.0
0.01
99.99
L
87.92
0.03
12.05
(Al)
98.5
0.0
1.5
(Si)
0.0
0.0
100.0
AlB2
33.3
66.7
0.0
Landolt‐Bo¨rnstein New Series IV/11E1
5
. Fig. 1 Al-B-Si. Reaction scheme
Al–B–Si
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
7
8
5
Al–B–Si
. Fig. 2 Al-B-Si. Liquidus surface projection
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Si
5
. Fig. 3 Al-B-Si. Isothermal section at 1300˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
9
10
5
Al–B–Si
. Fig. 4 Al-B-Si. Isothermal section at 500˚C
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Si
5
. Fig. 5 Al-B-Si. Partial temperature-composition section at 0.2 at.% B
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
11
12
5
Al–B–Si
References [1964Mat] [1969Lam]
[1972Lam]
[1977Hig] [1981Por]
[1982Doe]
[1983Hig] [1984Ole] [1990Luk]
[1994Dus] [1996Gro] [1998Fri]
[1999Wan] [2001Mes]
[2000Wan] [2003Nog] [2004Mir]
[2005Gro]
[2005Hui] [2005Yos1]
[2005Yos2]
Matkovich, V.I., Economy, J., Giese, R.F., “Presence of C in Al Borides”, J. Am. Ceram. Soc., 86, 2337–2340 (1964) (Crys. Structure, Experimental, 14) Lamikhov, L.K., Neronov, V.A., Rechkin, V.N., Samsonova, T.I., “On the β-AlB12 Phase in the Si-Al-B System” in org. Mater. (Engl. Trans.), 5, 1034–1036 (1969), translated from Izv. Akad. Nauk SSSR, Neorg. Mater., 5(7), 1214–1217 (1969) (Experimental, Morphology, 12) Lamikhov, L.K., Neronov, V.A., Rechkin, V.N., Samsonova, T.I., “β-AlB12 Phase in the Si-Al-B System” (in Russian), in “Metalloterm. Metody Poluch. Soedin. Splavov”, Kornilov, A.A. (Ed.), Nauka, Sib. Otdel. Novosibirsk, 52–57 (1972) (Review, Crys. Structure, 12) Higashi, I., Sakurai, T., Atoda, T., “Crystal Structure of α-AlB12”, J. Solid state Chem., 20, 67–77 (1977), (Experimental, Crys. Structure, 21) Portnoy, K.I., Bogdanov, V.I., Mikhailov, A.V., Fuks. D.L., “Interaction Parameters in Interstitial Solid Solutions Based on Aluminium”, Russ. J. Phys. Chem. (Engl. Transl.), 55(4), 583–584 (1981), translated from Zh. Fiz. Khim., (55), 1041–1043 (1981) (Experimental, 10) Doerner, P., “Constitutional Investigations on High Temperature Ceramics of the B-Al-C-Si-N-O System by Means of Thermochemical Calculations” (in German), Thesis, Uni. Stuttgart, Inst. Metallkunde, (1982) (Calculation, Thermodyn., 126) Higashi, I., “Aluminum Distribution in the Boron Framework of γ-AlB12”, J. Solid State Chem., 47, 333–349 (1983) (Experimental, Crys. Structure, 21) Olesinski, R.W., Abbaschian, G.I., “The B-Si System”, Bull. Alloy Phase Diagrams, 5, 478–484 (1984) (Review, Phase Diagram, 51) Lukas, H.L., “Aluminium - Boron - Silicon”, MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.20852.1.20, (1990) (Crys. Structure, Phase Diagram, Assessment, 6) Duschanek, H., Rogl, P., “The Al-B (Aluminum-Boron) System”, J. Phase Equilib., 15, 543–552 (1994) (Assessment, Crys. Structure, Phase Relations, Review Thermodyn., 78) Gro¨bner, J., Lukas, H.L., Aldinger, F., “Thermodynamic Calculation of the Al-Si-C System”, Calphad, 20, 247–254 (1996) (Calculation, Phase Diagram, Thermodyn., 37) Fries, S.G., Lukas, H.L., “B-Si” in “COST 507. Thermochemical Database for Light Metal Alloys”, Vol. 2”, Ansara, I., Dinsdale, A.T., Rand, M.H. (Eds.), Office for Official Publications of the European Communities, Luxembourg, 126–128 (1998) (Calculation, Phase Diagram, Thermodyn., 0) Wang, Li., Bian, Xiufang, Sun, Yimin, “Refining Effect of Boron on Hypoeutectic Al-Si Alloys”, Chin. J. Nonfer. Met., 9(4), 714–718 (1999) (Experimental, Morphology, 13) Meschel, S.V., Kleppa, O.J., “Thermochemistry of Alloys of Transition Metals and Lanthanide Metals with some IIIB and IVB Elements in the Periodic Table”, J. Alloys Compd., 321, 183–200 (2001) (Experimental, Thermodyn., 82) Wang, Li, Bian, Xiufang, “Refining Effect of Boron on Hypoeutectic Al-Si Alloys”, J. Mater. Sci. Technol., 16(5), 517–520 (2000) (Experimental, Morphology, 7) Nogita, K., Dahle, A.K., “Effects of Boron on Eutectic Modification of Hypoeutectic Al-Si Alloys”, Scr. Mater., 48(3), 307–313 (2003) (Kinetics, Morphology, 16) Mirkovic, D., Gro¨bner, J., Schmid-Fetzer, R., Fabrichnaya, O., Lukas, H.L., “Experimental Study and Thermodynamic Re-assessment of the Al-B System”, J. Alloys Comp., 384, 168–174, (2004) (Experimental, Assessment, Calculation, Phase Diagram, Phase Relations, Thermodyn., 26) Groebner, J., Mirkovic, D., Schmid-Fetzer, R., “Thermodynamic Aspects of Grain Refinement of Al-Si Alloys Using Ti and B”, Mater. Sci. Eng. A, 395(1-2), 10–21 (2005) (Assessment, Calculation, Phase Diagram, Phase Relations, Thermodyn., 56) Huiyuan, G., Yanxiang, L., Xiang, C., Xue, W., “Effects of Boron on Eutectic Solidification in Hypoeutectic Al-Si Alloys”, Scr. Mater., 53(1), 69–73 (2005) (Experimental, Morphology, 8) Yoshikawa, T., Morita, K., “Thermodynamic Properties of B in Molten Si and Phase Relations in the Si-Al-B System”, Metal. Trans., 46(6), 1335–1340 (2005) (Experimental, Phase Relations, Thermodyn., 16) Yoshikawa, T., Morita, K., “Removal of B from Si by Solidification Refining with Si-Al Melts”, Metal. Trans. B, 36(6), 731–736 (2005) (Experimental, Phase Relations, 18)
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–B–Si [Mas2] [V-C2]
5
Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_5 ß Springer 2009
13
Al–C–Ti
6
Aluminium – Carbon – Titanium Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Lesley Cornish, Gabriele Cacciamani, Damian M. Cupid, Jozefien De Keyzer
Introduction Al-C-Ti alloys are of interest for many different reasons, mainly as alloys in themselves, dispersion-hardened alloys with TiC, and also as grain refiners for commercial Al-based alloys, giving improved properties. Alloys are based on Ti-6Al/TiC [2002Zha2], which has high strength, low density and good elastic modulus. Ti3Al and γαffl (TiAl) phases are being developed for lightweight structural applications, especially at elevated temperatures. The system is also important for composite manufacture; using TiC in (Al), and also using the ternary carbides. Ti2AlC is recognized as a “machinable ceramic”, its layered structure produces a combination of metallic and ceramic properties. Additionally, there is interest for coatings: Ti-Al-C PVD coatings could compete with Ti-Al-N, and in a different application, TiC has potential for a barrier diffusion layer for silicon semiconductor devices. Phase boundary information on this system comes from the work of [1954Thy, 1980Sch, 1987Zak], [1989Cam1, 1989Cam2, 1991Cam1, 1991Cam2, 1992Pie, 1994Pie] mostly using optical and electron microscopy together with and X-ray diffraction. Other publications [1963Jei, 1964Jei, 1964Now, 1976Ivc1, 1976Ivc2, 1980Pea] covered X-ray diffraction studies, crystal structures, lattice parameters and physical properties of the two ternary carbides Ti2AlC and Ti3AlC, with general agreement. One of the first reviews was by [1965Mol], followed by [1983Kub, 1983Sri]. The first evaluation within the ongoing MSIT Evaluation Program was made by [1990Hay], which is updated by the present work. Recent reviews by [1994Pie, 2000Ban, 2006Rag] (where [1994Pie] also undertook experimental work) mainly include the experimental information obtained after the original MSIT review of [1990Hay]: [1990Via, 1991Cam1, 1992Pie, 1994Pie, 1994Zha]. Information of some other recent articles that were not considered there ([1990Hay]) are included in this review [1991Cam2, 1995Via, 2000Ria, 2000Tze, 2000Van, 2003Ge1, 2005Zho2]. An overview of the investigations considering phase equilibria, solid phases and thermodynamics of the system is given in Table 1.
Binary Systems For the Al-Ti system, the MSIT evaluation from [2004Sch] is available. More recently, a new review of [2006Sch] and a thermodynamic assessment of [2007Wit] appeared which show differences in two main regions. [2006Sch] and [2007Wit] consider the equilibria between (αTi), (βTi) and Ti3Al. Starting from the same experimental literature information, [2004Sch] concluded that Ti3Al decomposes congruently and there is no invariant equilibrium involving Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
1
2
6
Al–C–Ti
these three phases, while [2006Sch] and [2007Wit] concluded that there are two peritectoid reactions between these three phases and a small two-phase field between (βTi) and Ti3Al in the 1150˚C-1200˚C temperature range. According to [2004Sch], the different phase equilibria may be related to very small differences in Gibbs energy, and consequently in driving forces, to give the possible phase transitions in that range. Thus, it is very difficult to decide which interpretation of the experimental data is actually correct. The second difference considers the equilibria between γ(TiAl), TiAl2 and one-dimensional antiphase domain structures or “long period structures (LP)” stable at high temperature in the range between 65 and 75 at.% Al. In this case, the assessments by [2006Sch] and [2007Wit] are based on more recent experimental data and give a more complete discussion of the stable equilibria in this region. Thus the phase diagram calculated by [2007Wit] is accepted in the present evaluation since it is based on experimental data available, the majority of which were assessed in [2006Sch], being complemented by own key experiments. The adopted Al-Ti phase diagram is shown in Fig. 1 from [2007Wit]. The Al-C phase diagram is accepted from the review of [2004Per]. The C-Ti phase diagram (Fig. 2) is taken from the recent thermodynamic calculation of [2003Fri]. It leads to a better fit of high temperature heat capacity measurements than all previous studies. The phase diagram of [2003Fri] is reproduced with the same accuracy as given by [1999Dum] and gives a better description of the experimental data than previous assessments. However, it should be noticed that the liquidus lines are not supported by any experimental data.
Solid Phases The solid phases are given in Table 2. The different morphologies of TiAl3 are deemed to be related to the different morphologies observed at different cooling rates and Ti contents [1982Bla, 1993Sve]. Similarly, TiAl2 has been reported to have metastable structures in ascast alloys [2001Bra]. The Ti2Al5 phase [2004Sch] is interpreted here as a one dimensional antiphase domain structure or “long period structure (LP)” stable at high temperature in the range between 65 and 75 at.% Al. The Ti5Al11 phase has been included in Table 2, although it is not accepted here as a separate phase, and is presumed to be related to ζ, Ti2Al5, with which it shares similar lattice parameters. According to [1989Cam1, 1989Cam2], carbon solubilities in the binary aluminides are small (~1 at.% C) and the absence of fine scale carbide precipitates after ageing the alloys with 1 at.% C for 15 days at 750˚C and 450˚C respectively shows the absence of a significant decrease of C solubility in (αTi) or Ti3Al [1989Cam1, 1989Cam2]. Ternary carbides are stated to form above 1250˚C by peritectic reactions from TiC1–x and liquid. All workers have reported minimal solubility of aluminium in TiC1–x [1984Ker, 1980Sch, 1989Cam1, 1989Cam2, 1990Cam, 1991Cam1, 1991Cam2, 1994Pie, 2000Ria]. [1980Sch] confirmed the existence of the hexagonal ternary H-phase Ti2AlC and of the cubic Perovskite-(P-) phase Ti3AlC reported by earlier workers [1963Jei, 1964Jei, 1964Now, 1976Ivc1, 1976Ivc2, 1980Pea]. A cubic phase that was earlier noted in a Ti-10Al-1C (mass%) alloy [1954Thy] probably was the cubic Perovskite-phase Ti3AlC; this was confirmed by [2000Ria], although [1994Pie] reported not being able to find a match. [1994Pie] found a third ternary phase, N, Ti3AlC2. It is presumed that the reason for this phase not being observed earlier was that longer sintering times and higher pressures [2006Li] were needed. DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
The ternary carbides have less C than their stoichiometric compositions [1980Sch, 1992Pie, 1994Pie, 2000Tze] and the range for N is at least Ti3Al1.1C1.8 [2000Tze] to Ti3Al1.1C2.3 [2005Kho]. The relationship of TiC1–x and Ti2AlC1–x to Al4C3 was discussed by [1982Now]. The unusual diffusion path reported by [1995Via] between (Al) and TiC could possibly have been due to the then unrealized N phase.
Quasibinary Systems The section between γ (TiAl) and TiC1–x by [1987Zak] is not a true quasibinary since both peritectic reactions have a (non-linear) three-phase field.
Invariant Equilibria The invariant reactions are not fully derived yet, and more work needs to be done. The agreed invariant equilibria of [1991Cam1, 1994Pie] are given in Table 3. Ti2AlC melts incongruently at 1625±10˚C; Ti3AlC also melts incongruently at 1580±10˚C, whereas Ti3AlC2 decomposes in the solid state [1994Pie]. [2004Hwa] observed that ternary carbides formed from peritectic reaction with TiC1–x ; this confirmed the reaction: L + TiC1–x Ð H of [1987Zak], which [1994Pie] reported having a maximum at 1625±10˚C. [1992Che] deduced that cubic Ti3AlC is a metastable transition phase which is ultimately replaced by the more stable H (Ti2AlC) phase, which agrees with the reactions of [1994Pie]. According to [2005Zho2], the lower stability limit of Ti3AlC2 is ~1300˚C (decomposing to give TiC1–x and Al vapor) and [2000Tze] reports the upper stability limit as at least 1400˚C, if not 1450˚C. The most Al rich equilibrium in Table 3 is from [1990Via, 1993Sve], where the latter deduced that the formation kinetics of Al4C3 were slow, and the reaction agreed with [1998Fra]. [1990Via] gave alternative Al rich reactions: L + Al4C3 + TiAl3 Ð (Al) or L + TiAl3 Ð Al4C3+ (Al), both being very near to the melting point of aluminium.
Liquidus, Solidus and Solvus Surfaces [1991Cam1] derived a “semi-schematic” liquidus surface. The volume fraction of H was less than the projection suggested; this was thought to be due Al substituting for C. A schematic liquidus surface and partial reaction scheme was also derived by [1994Pie]. They are not presented here, since they contain extra Al-Ti phases which are not accepted in this review. However, the liquidus surface is dominated by TiC1–x , then graphite. The reactions forming the other phases all lie very close to the Al-Ti binary. [1990Via] gave an experimental liquidus projection in the Al rich corner, whereas [1998Fra] produced one from thermodynamic calculations. The major difference was that [1990Via] gave the lowest temperature reaction, which was dependent on cooling conditions. [1993Sve] also attempted to rationalize the different morphologies of TiAl3 observed with composition.
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
3
4
6
Al–C–Ti
Isothermal Sections [2003Ge1] drew an isothermal section at 1300˚C showing the third ternary phase, N (Ti3AlC2), which was involved in the three-phase triangles: (N + H + TiC1–x), (N + TiC1–x + TiAl3) and (N + H + Ti5Al11), but the last phase (as well as its Al-Ti phase diagram) is not accepted here. Additionally, the phase compositions did not agree with the boundaries due to Al loss. Similarly, the isothermal section at 1300˚C of [1992Pie, 1994Pie] is not presented. The 1100˚C isothermal section of [1994Zha] is not presented because it contains Ti2Al5 which is not accepted here, although it mainly agrees with the other sections presented. [2000Ban] gave isothermal sections at 1300, 1100 and 1000˚C, but these are not reproduced because they are incompatible with the Al-Ti binary accepted here, and show a radical change in the positions of the P and H ternary phases over the temperature ranges (especially 1100˚C). [1993Tia] established a metastable diagram between 900 and 1050˚C. The isothermal section at 1250˚C was drawn by [1991Cam1], and is shown in Fig. 3 after modifications to be consistent with the accepted Al-Ti binary. [2000Ria] modified the 1050˚C isothermal section of [1990Cam], with additional results that retained the same phase fields, but changed the shape of some of them, notably ((αTi) + P + TiC1–x). This is redrawn in Fig. 4 to be consistent with the Al-Ti binary system accepted here, the positions of the P and H, and keeping their alloys in the respective phase fields. The redrawn P and H phases in Figs. 4 and 1 are also consistent with those of [1990Via], but the isothermal sections of [1990Via] are not given here because negligible solubility is given for all binary phases. The results of [1954Thy] and [1989Cam1, 1989Cam2, 1991Cam1] indicate that both (αTi) and (βTi) solid solutions are in equilibrium with TiC, thus generating the tie-triangles ((αTi) + (βTi) + TiC) and ((αTi) + TiC + P) (Fig. 5) at 1000˚C. This is taken rather than the Ti rich corner of [1980Sch], which showed that at 1000˚C, (βTi) solid solution is in equilibrium with the Perovskite carbide phase Ti3AlC (P) generating the two tie-triangles ((βTi) + TiC + P) and ((αTi) + (βTi) + P). This decision was made because [1980Sch] showed those relationships as dotted, and did not give the sample compositions. Their drawn phase relationships also contradict their statement that (βTi) was not retained in the ternary. Additionally, seven experimental alloys of [1994Zha] agree with the findings and interpretation of all previous workers, except for [1980Sch]. There is agreement that γαffl (TiAl) is in equilibrium with Ti2AlC at 1000˚C [1980Sch, 1987Zak, 1989Cam1, 1991Cam1]. The isothermal section at 750˚C (Fig. 6) is taken from [2000Ria], but redrawn to be consistent with the Al-Ti binary accepted here (Fig. 1), the positions of the P and H, as well as the low carbon solubilities reported in the Al-Ti phases, except for (αTi) [1954Thy, 1980Sch, 1987Zak, 1989Cam1, 1989Cam2, 1991Cam1, 1991Cam2, 1992Pie, 1994Zha]. This is consistent with the isothermal section at 1000˚C in terms of reduced ternary element solubilities in the phases at lower temperatures. The section of [2000Ria] is preferred to that of [1991Cam1] because it was derived using alloys further into the ternary system (up to 15 at.% C) [2000Ria], instead of only up to 3 at.% C [1991Cam1]. The redrawing of the diagram brings the only contentious alloy of [1991Cam1] to a position nearly on the boundary between the ((αTi) + TiAl3 + P) and ((αTi) + P + TiC1–x), which could explain why P was not found. Although it appears that TiC1–x [1991Cam1] was re-precipitated within the grains, it would have been the primary phase [1994Pie] and [1995Via] has shown that it takes a long time to disappear. In the isothermal sections presented, the compositions of the P and H phases were modified to agree with those of the 1000˚C isothermal section since this was the widest ranges, and DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
otherwise the other sections had compositions which fell outside this range, especially those of [2000Ria] which used higher Ti content alloys. Experimental work on liquid (Al) by [1993Sve] showed that there were three-phase regions: ((Al) + TiAl3 + TiC1–x) and ((Al) + Al4C3 + TiC1–x). Several calculations have been undertaken on the Al rich corner: [1998Fra] showing the equilibrium between (Al) with TiC1–x and TiAl3 and [2000Van] which confirmed [1998Fra], while studying grain refiners.
Temperature – Composition Sections Isopleths for the concentration range 0–1 mass% C at 2, 4, 6, 8 and 10 mass% Al were determined by [1954Thy] and boundaries between the following phase fields were located: (αTi), (βTi), ((αTi) + (βTi)), ((βTi) + TiC1–x), ((αTi) + (βTi) + TiC1–x) and a field containing more than one phase one of which is TiC1–x. The solubility of C in (αTi) was found to increase with increasing Al contents rising to over 1 mass% C at 1150˚C and 10 mass% Al. These are reproduced in Figs. 7–11) from [1990Hay] who redrew them slightly (but without compromising the original experimental results) to be consistent with isothermal sections, and they are redrawn slightly to be consistent with the adopted Al-Ti binary. A section at 0.2 at.% C [1997Li, 1999Li] agrees with the accepted binary. [1987Zak] derived a γ(TiAl)TiC1–x section (Fig. 12).
Thermodynamics [1986Ban] determined the Gibbs free energy of formation of the compounds Al4C3 and TiC as a function of temperature in the range 300–1800 K. The same was calculated by [1991Rap] in order to demonstrate that the formation of Al4C3 is metastable with respect to TiC and it is due to kinetic reasons. Thermodynamics and kinetics of formation of TiC by a reaction between Al-Ti melts and a carbonaceous gas have been studied by [1991Sah]. More recently [2006Ton] used thermodynamic analysis to show that it is feasible to produce TiC-Al (Ti) nanocomposite powders using Al and Ti as starting materials and CH4 as reacting gas in a thermal plasma environment. Based on thermodynamic results previously available in literature, [1991Yok] presented a three-dimensional potential phase diagram for the Al-C-Ti system at 700˚C. [1993Jar] investigated thermodynamics and kinetics of the reactions taking place during infiltration of graphite fibres by molten Al-Ti alloys. A temperature range for safe processing of Al-TiC composites has been suggested by [1993Mit] based on thermodynamic considerations. [1993Sve] determined by a theoretical thermodynamic analysis the C and Ti concentration in Al-rich liquid in equilibrium with solid phases at temperatures between 700 and 1100˚C. A thermodynamic discussion of the solid/liquid phase equilibria in the Al rich corner has been reported also by [1998Fra]. Limiting values of thermochemical data of formation of the Al-C-Ti ternary compounds are reported in [1994Pie], based on binary and ternary Al-C-Ti equilibria and thermochemical data for various reactions previously studied in literature. The authors concluded that the dataset so obtained was sufficient to calculate tie lines in agreement with known phase equilibria but a full thermodynamic assessment of the system is needed. Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
5
6
6
Al–C–Ti
Thermodynamics of formation of TiC in DC-casting and melt spun Al-C-Ti alloys has been discussed by [1994Ton]. Thermodynamics and kinetics of formation of TiC in Al-C-Ti have also been investigated by [2000Zha2]. Thermodynamics and kinetics of precipitation of TiC in Al-C-Ti melts at 1100˚C have been investigated by [1999Jar]. Low temperature heat capacity of Ti3Al1.1C1.8 has been measured by [1999Ho]. Heat capacity, thermal expansion coefficients and thermal conductivity of the Ti2AlC phase have been measured by [2002Bar] at room to high temperature: these are reported in Table 4. Low temperature heat capacity of the same phase has been measured by [2006Dru].
Notes on Materials Properties and Applications The work on materials properties is summarized in Table 5. The system is of interest because of the effect of different additions to the grain refining of many commercial Al-based alloys [1949Cib], with the benefits of improved mechanical properties, reduced ingot cracking, improved feeding and increased casting speeds, improved homogeneity and reduced porosity and better deformation behavior. Grain refiners based on Al-C-Ti can be added in master alloy form, and are an alternative to conventional Al-B-Ti grain refiners [1994May] and are less susceptible to agglomeration. [1976Jon] calculated solubility limits of liquid aluminium in different systems, including Al-C-Ti. Epitaxy was found to be important; thus TiC was seen as being more effective than TiAl3, having more epitaxial faces [1972Cis]. However, TiC is surrounded by Al4C3, then Ti3AlC, which reduces the grain refinement effectiveness, and so heating liberates the beneficial TiC [1986Ban]. Several studies were made on the formation of the grain refining precipitates [1977Ivc, 1989Cam1, 1991Fro, 1991Sah, 2000Bri1, 2000Zha1, 2002Zha1, 2003Zha2], to improve the methods [2000Zha1, 2005Zha, 2005Kum] and to assess the efficiency [2000Bri2, 2000Rom, 2000Sch, 2000Van, 2002Gaz, 2002Tro, 2002Xia, 2002Liu, 2003Zha2]. Aluminium alloys grain refinement has also been achieved by synthesizing Al-Ti-C launders and moulds in an electromagnetic field [2005Xia]. There are also several alloys based on Ti-6Al/TiC1–x [2002Zha2] which have high strength, low density and good elastic modulus. Aluminium dispersion-hardened alloys are also important and different alloys in different conditions have been studied: up to 50 mass% TiC1–x [1986Bat]. The Ti3Al and γ (TiAl) phases are being developed for lightweight structural applications, especially at elevated temperatures. γ (TiAl) is disadvantaged by low temperature ductility and toughness, and these are being improved by precipitation [1991Mab]. Composites are also being developed by precipitating Ti3AlC in HIPped γαffl (TiAl) alloys [1992Che, 1994Whi], although the precipitate long-term stability was questioned [1992Che]. Optimization of the lamellar microstructural has been attempted [2001Qin]. Improvements have also been made by indirect-extruding TiAl-Mn-Mo-C alloys to obtain a fine microstructure, and rheocasting TiAl alloys and composites [1997Ich]. The system is also important for composite manufacture; composites have been made by infiltrating graphite fibres with molten Al-Ti, using the phase diagram [1993Jar]. In-situ internal carburization has also been carried out to fabricate the composites [1991Jar, 1999Bir, 2001Zha]. [1995Mor] made in-situ TiC1–x particulate reinforced aluminum composites by reacting graphite particles in a liquid Al-Ti alloy and showed that the Young’s modulus and tensile strength increased proportionally to the TiC1–x volume fraction. Ductile Al/TiC DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
MMCs (metal matrix composites) have also been made [1993Mit, 2003Arp] and the effects of the TiC1–x dendrite spacing were studied [2002Ria]. Bulk [2004Hwa, 2004Wan3, 2005Jia, 2005Li, 2006Xia] and porous [1992Vol] Al-C-Ti cermets have also been manufactured using the SHS (self-propagating high-temperature synthesis) sintering technique [1992Vol, 1997Lee, 1997Ye, 2002Mei, 2006Xia] and phase evolution studied [2005Rog]. Variations of thermal explosion/quick pressure (TE/QP) methods have also been used [2001Yan, 2005Ma], and “hot shock” [1998Tan]. Combustion synthesis, also known as self-propagating high-temperature synthesis (SHS), offers advantages of low processing cost, energy-efficiency, and high production rate, and has been used to manufacture TiC1–x [1993Cho, 2006Xia]. Addition of synthesized master alloys to molten aluminium has also been achieved [2006Sel], and a dipping exothermic reaction process (DERP) has also been used [2003Son, 2004Son2]. [1996Tom] produced ternary composites by combustion synthesis with titanium, aluminium, and graphite powders. At low C-contents, binary intermetallics were formed, whereas Ti2AlC and TiC1–x were formed at higher C-contents. Other elements have also been added to the materials [2003Yan]. A useful review of these and other composites is [2000Tjo]. Some of the composites are being developed for cutting tools [1967Hod, 1976Ivc1], using the intermetallic phases, and TiC1–x shows the most promise. An extension of this are complex carbides (or nitrides) M2AlC (or N), where M = Cr, Ti, V, Nb or Ta [1996Cha]. Also, the system has been considered for coatings on Ti-based metal matrix composites containing alumina fibres [1994Din]. Studies have been made of solid state reactions at graphite/TiAl or Ti3Al interfaces, showing that whilst graphite moulds are safe for these alloys, carbon fibres would have to be coated to prevent Ti diffusion [1995Via]. Ti2AlC is recognized as a “machinable ceramic” (layered structure) with good mechanical properties and low thermal expansion, thus giving potential high temperature applications (furnace apparatus). It has been manufactured by self-propagating high-temperature synthesis (SHS) [2001Lop], combustion synthesis [2004Kex], “thermal explosion” (a form of SHS) [2002Kho1, 2002Kho2], hot pressing [2004Hon, 2005Pen], spark plasma sintering [2003Zho, 2004Mei, 2005Zho1], two-stage pressureless sintering followed by hot pressing [2005Wan1]. Similarly, interest has also been shown in Ti3AlC [2001Lop] and Ti3AlC2 [2000Tze, 2001Lop, 2003Ge1, 2003Ge2, 2004Son1, 2005Kho, 2005Zho2, 2006Li], with similar manufacturing processes. Ti3AlC pins twins in γ (TiAl) [1997Chr]. Ti-Al-C PVD coatings have been manufactured as possible competitors to Al-N-Ti coatings [1991Kno] and for coatings for steels [2005Wal]. Another coating application is as a diffusion barrier for materials in contact structures for silicon semiconductor devices. Aluminium can be used (rather than the more effective and expensive PtSi), but needs a barrier diffusion layer, and this can be TiC1–x [1982Wit].
Miscellaneous The formation mechanism for TiC1–x from the ball-milled elemental components was studied by [2003Wan2]. Various reaction mechanisms for combustion reactions to yield TiC1–x [1993Cho] (with results of the first TiC formation supported by [1995Via]), Ti3AlC2 [2002Ge], and TiC / γ(TiAl) composites [2002Hwa] have been proposed. [1993Cho] studied the effect of Al addition (0-40 mass%) on the combustion reaction between Ti and C to form TiC1–x using combustion wave velocity data and differential thermal analysis. Their results Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
7
8
6
Al–C–Ti
indicate the reaction between titanium and aluminium initiates the reaction between titanium and carbon through a series of reaction steps. [2002Hwa] also used combustion synthesis to create TiC1–x/Al composites, but reported the presence of ternary carbides in the final microstructure. In-situ processing of aluminium matrix metal matrix composites based on TiC has been investigated [1995Mor, 1996Tom, 1993Ber]. [1996Mat] performed electronic structure calculations for C-containing γ (TiAl) and showed that C substitutes Al sites. [1996Ily] undertook electronic structure calculations on Ti1–xAlxC (x = 0.17), and showed that this compound has a bandgap of 2.18 eV. Ab-initio electronic structure calculations were performed on C-containing γ (TiAl) [1996Mat] and on theoretical Ti1–xAlxC compounds (NaCl lattice where Al and Ti occupy the same lattice sites) by [1996Ily, 1997Ily1, 1997Ily2, 1998Mat]. The wetting angle of molten Al on TiC1–x was measured using the sessile drop method by [1966Yas] at 117˚. [1996Sob] used the same method to investigate the wettability of Al-rich Al-Ti alloys (Al-0.5Ti to Al-10Ti (mass%)) and showed that Ti additions lead to better wettability of graphite because of reactions between titanium and carbon. Gibbs free energy calculations [1994Ton, 1996Tom, 1995Mor] have been used to predict/ determine reactions and phase stabilities for aluminium-based metal matrix composites with Ti and C. [1997Wu] ball milled titanium, aluminium, and graphite powders in the atomic ratio Al-0.23Ti-0.23C and produced an amorphous phase that further transformed to an fcc metastable phase. Annealing at 600˚C for 45 minutes yielded the equilibrium phases (Al), Al3Ti and TiC1–x(?).
. Table 1 Investigations of the Al-C-Ti Phase Relations, Structures and Thermodynamics
Reference
Method/Experimental Technique
Temperature/ Composition/Phase Range Studied
[1954Thy]
Optical metallography and XRD
0-1 mass% C at 2, 4, 6, 8 and 10 mass% Al
[1963Jei]
Powder metallurgy, XRD
Ti2AlC
[1964Jei]
Powder metallurgy, XRD
Ti3AlC
[1964Now]
Powder metallurgy, XRD
Ti2AlC
[1972Now]
Powder metallurgy, XRD
Ti2AlC
[1976Ivc2]
Powder metallurgy, XRD
Ti2AlC and Ti3AlC
[1977Gur]
Metallography, XRD, magnetic properties TiAl2.97C0.03 measurements
[1980Pea]
Dimensional analysis
Ti2AlC
[1980Sch]
XRD
1000˚C; 30 alloys of nonspecified composition
[1984Ker]
Metallography, SEM and EDS.
Solubility of Al in TiC1–x at 1600˚C
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Table 1 (continued)
Reference
Temperature/ Composition/Phase Range Studied
Method/Experimental Technique
[1987Zak]
Metallography and X-ray diffraction
600˚C - 1400˚C, TiAl-TiC, up to 25 mass% TiC0.98
[1993Tia]
XRD, TEM
(Ti0.50Al0.50)99.5C0.5
[1989Cam1, 1989Cam2, 1990Cam, 1991Cam1, 1991Cam2]
Light microscopy, SEM, TEM, X-ray diffraction, X-ray ED spectroscopy, EDX and hardness measurements
750˚C, 1000˚C, 1250˚C, 15 < at.% Al < 55, 0.5 < at.% C <3
[1999Far]
TEM, HRTEM
Ti3AlC2
[1992Aye]
SEM, WDS and EDS on HIPped ingots
Ti2AlC1–x
[1992Pie, 1994Pie]
X-ray diffraction
1100˚C, 900˚C and 700˚C
[1993Sve]
Light optical microscopy, SEM, EDS
1100˚C, 900˚C and 700˚C / Low C and up to 2.22 at.% Ti / Liquid (Al), Al4C3 and TiC1–x
[1995Via]
Diffusion couples, X-ray diffraction
1000˚C
[1997Li, 1999Li]
EPMA
Ti46Al-0.2C
[2000Ria]
SEM, TEM, X-ray diffraction
750˚C, 1000˚C
[2005Wan3]
XRD
Ti3AlC2, Ti2AlC and TiC1–x
[2006Lin]
XRD, TEM with EDS, HRTEM
Ti2AlC
. Table 2 Crystallographic Data of Solid Phases Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
(βAl)
hP2 P63/mmc Mg
a = 269.3 c = 439.8
at 25˚C, 20.5 GPa [Mas2]
(αAl) < 660.452
cF4 Fm3m Cu
a = 404.96
at 25˚C [Mas2]
(C)d
cF8 Fd3m C (diamond)
a = 356.69
at 25˚C, 60 GPa [Mas2]
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
9
10
6
Al–C–Ti
. Table 2 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
(C)gr < 3827
hP4 P63/mmc C (graphite)
a = 246.12 c = 670.90
at 25˚C [Mas2] sublimation point
(ωTi)
hP3 P6/mmm ωTi
a = 462.5 c = 281.3
at 25˚C, HP at 1 atm [Mas2]
(βTi) 1670 - 882
cI2 Im3m W
a = 330.65
pure Ti [Mas2]
-
Possible ordering from A2 (βTi) to B2 (β0) [2000Ohn]
a = 295.06 c = 468.35
at 25˚C [Mas2]
cP2 β0, (βTi,Al) ~1427 - ~1104 Pm3m CsCl (αTi) < 882
hP2 P63/mmc Mg
α2, Ti3Al < 1193 (up to 10 GPa at RT)
hP8 P63/mmc Ni3Sn
γ, TiAl < 1456
a = 578.83 c = 463.7 a = 580.6 c = 465.5 a = 574.6 c = 462.4
tP4 P4/mmm AuCu
a = 400.0 c = 407.5 a = 398.4 c = 406.0
D019 ordered phase [1997Sah] [1980Sch]
at 22 at.% Al [L-B] at 38 at.% Al [L-B] L10 ordered phase, has c/a > 1 50 at.% Al at 1000˚C [2001Bra] 62 at.% Al at 1100˚C [2001Bra]
Ti1–xAl1+x > 1170
tP4 P4/mmm AuCu
a = 403.0 c = 395.5
Ti3Al5 < 809
tP32 P4/mbm Ti3Ga5
a = 1129.3 Ti3Al5, stable below 810˚C [2001Bra] (a = 399.3 substructure) c = 403.8
ζ, Ti2Al5 1432 - 976
tP28 P4/mmm Ti2Al5
a = 393.6 c = 413.54
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
Disordered Ti1–xAl1+x has c/a < 1 [2001Bra], and was reported as a separate high temperature phase
[1986Mii] Presumed ordering effect
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Table 2 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm] a = 398.0 c = 2436.0
Comments/References
TiAl2 < 1224
tI24 I41/amd HfGa2
Ti5Al11 ≥ 995
CuAu a = 395.3 superstructure c = 410.4
[2001Bra] 1300˚C, but not recognized here as a separate phase
ε(h), TiAl3 (h) 1396 - 734
tI8 I4/mmm TiAl3(h)
[V-C2]
a = 384.6 c = 859.4
[1980Mii, 1986Mii] by TEM
a = 384.9 1000˚C [2001Bra] c = 860.9 (c = 430.5 substructure)
ε(l), TiAl3 (l) < 932
tI32 I4/mmm TiAl3(l)
a = 387.7 76 at.% Al at 640˚C [2001Bra] c = 3382.82 (c = 422.9 substructure)
TiC1–x
cF8 Fm3m NaCl
a = 432.8
[V-C2]
Al4C3
hR21 R3m Al4C3
a = 333.8 c = 2511.7
[V-C2]
* H, Ti2AlC1–x
hP8 P63/mmc Cr2AlC
a = 305.6 c = 1362.3
[V-C2]
* P, Ti3AlC1–x
cP5 Pm3m CaTiO3
a = 415.6
[V-C2]
* N, Ti3AlC2
hP12 P63/mmc CMo
a = 307.53 c = 1857.8
[1994Pie], isotypic with Ti3SiC2
Metastable / high pressure phases TiAl3 (m)
cP4 Pm3m AuCu3
Ti3Al (I) hP16 15 to > 41 GPa P63/mmc TiNi3
Landolt‐Bo¨rnstein New Series IV/11E1
a = 397.2
Splat cooled; 85 at.% Al [1994Bra]
a = 531.2 c = 960.4
[1997Sah] at 16 GPa; Not found at 0–35 GPa, 25-2250˚C [2004Sch]
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
11
12
6
Al–C–Ti
. Table 2 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
TiAl2 (m)
oC12 Cmmm ZrGa2
a = 394.21 c = 401.61
~66 to 67 at.% Al - metastable in as-cast alloys [2001Bra]
Ti52Al48 (m)
cP20 P4132 βMn
a = 690
Precipitated in amorphous thin film after 1 h at 525˚C [1999Abe]
. Table 3 Invariant Equilibria Composition (at.%) T [˚C]
Reaction
Type
Phase
Al
C
Ti
L + TiC1–x + H Ð P
1580±10
P
-
-
-
-
L + TiC1–x Ð (βTi) + P
1430 < T < 1580
U
-
-
-
-
L + P Ð (βTi) + H
Lower than the above
U
-
-
-
-
L + (βTi) Ð (αTi) + H
<1460
U
-
-
-
-
L + TiC1–x Ð TiAl3 + Al4C3
812
U
L
99.6281
0.0019
0.0019
. Table 4 Thermodynamic Properties of Single Phases
Phase
Temperature Range [˚C]
Property, per mole of atoms [J, mol, K]
Comments
Ti2AlC 30-1300
CP = 58.1+0.1·T–7·10–5·T2+ 1.8·10–8·T 3
[2002Bar]
Ti2AlC 30-1000
ktot = 49–0.01·T
thermal conductivity [2002Bar]
Ti2AlC 30-1000
TEC = 8.7·10
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
–6
–1
(K )
MSIT1
thermal expansion coefficient [2002Bar]
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Table 5 Investigations of the Al-C-Ti Materials Properties Reference
Method / Experimental Technique
Type of Property
[1967Hod]
Machining tests; microhardness measurements
Cutting tool ranking; microhardness
[1976Ivc1]
Electrical and thermal; microhardness measurements
Coefficients of thermal expansion; emf; electrical and thermal conductivities; microhardness of constituent phases
[1976Jon]
Optical microscopy, SEM and calculation
Grain refining capability
[1977Ivc]
Optical microscopy, SEM and DTA
Precipitate characterization and formation
[1982Wit]
Sputter coater, Rutherford backscattering and XRD
Coating characterization
[1986Ban, 2000Rom]
Powder metallurgy, optical microscopy, SEM and TEM
Precipitate characterization and formation for grain refining
[1986Bat]
Mechanical properties
Yield strength, elongation and hardness
[1989Cam1, 1989Cam2]
Optical microscopy, SEM and TEM with EDX, hardness measurements
Precipitate characterization and formation; hardness
[1991Fro]
Mechanical alloying, DSC, DTA, optical microscopy, and SEM with EDX and WDS
Precipitate characterization and formation
[1991Jar, 1992Jar, 1999Bir]
Crucible furnace, optical microscopy and XRD
Manufacture of TiC-(Al) composite; precipitate formation and characterization
[1991Kno]
PVD-coatings, SEM with EDX
Phase proportions
[1991Mab]
Reactive synthesis, arc-melting, compression testing, optical microscopy, TEM and XRD
Phase proportions; compressive strengths
[1991Sah]
Carrier gas, calorimetry and TEM Precipitate formation and characterization
[1992Che]
Powder metallurgy, reaction sintering, SEM, and TEM with EDX and EELS
Precipitate characterization and formation
[1992Cho, 1996Sun, 1999Zha, 2002Fra, 2002Kho2, 2003Ge1, 2003Ge2, 2005Ma]
SHS combustion chamber, XRD and SEM
Characterization and reaction temperatures
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
13
14
6
Al–C–Ti
. Table 5 (continued) Method / Experimental Technique
Reference
Type of Property
[1992Vol, 1997Lee, 1997Ye, Powder metallurgy, combustion 2002Hwa] reaction chamber (reaction sintering), optical microscopy, XRD, WDS and SEM
Formation and characterization of TiC precipitates
[1993Den]
Atom probe
Partitioning between γTiAl and Ti3Al3
[1993Ber, 1993Cho, 1993Jar, 1995Mor, 1995Via 1996Tom, 2002Ge, 2002Hwa]
Reaction between graphite and liquid Al-Ti alloy
Aluminum matrix metal matrix composites (In-situ)
[1993Cho, 2006Xia]
Combustion chamber, XRD and SEM with EDS
Manufacture and characterization of TiC-(Al) cermet
[1993Jar]
Infiltration, SEM with EDS
Precipitate characterization and formation
[1993Mit]
Casting; extrusion; microhardness tests; tensile tests; SEM, TEM and XRD
Formation and characterization of (Al)/TiC; microhardnesstemperature relationships; Young’s modulus, yield stress and elongation
[1993Tia]
TEM, mechanical tests
P/γTiAl orientation relationships; 0.2% proof stress
[1994Din]
HIP, XRD
Phase distribution
[1994May]
Optical microscopy, SEM, Precipitate characterization, (extraction replica) TEM with EDX formation and distribution and XRD
[1994Ton]
Rapid quenching
Precipitate formation, distribution and characterization
[1994Whi]
HIP, optical microscopy, SEM, TEM and XRD, compression, creep and tensile tests
Volume fraction; yield strength, UTS, elongation and ductility (RA); compressive strain, compressive creep curves
[1995Nuk]
Infiltration of preform, DTA and XRD
Formation reactions of TiC
[1996Mat, 1996Ily, 1997Ily1, Ab initio and structure 1997Ily2, 1998Mat, calculations 2001Zho1, 2001Zho2, 2003Wan1]
Electronic structure calculations
[1996Sob]
Sessile drop
Wettability of substrate with molten Al-Ti alloys
[1997Chr, 2005App]
TEM
Characterization of mechanically tested samples
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Table 5 (continued) Reference
Method / Experimental Technique
Type of Property
[1997Wu]
Mechanical alloying of titanium, aluminium, and carbon powder
Nanocrystalline phase formation
[1998Tan, 2000Bri1]
Reactive synthesis, DSC, optical microscopy, SEM and XRD
Formation, characterization and distribution of precipitates
[1999Far]
HRTEM
Characterization of Ti2AlC and Ti3AlC2
[2000Bar1]
HIP, XRD, mechanical tests
Characterization; coefficients of expansion
[2000Bri2, 2000Van]
Optical microscopy, XRD and SEM
Assessment of grain refining efficiency
[2000Fin]
Mechanical properties
Elastic properties of Ti3AlC2
[2000Ken]
Powder metallurgy, XRD, SEM
Formation and characterization of precipitates
[2000Zha1]
XRD, chemical analysis, SEM with Precipitate characterization, EDS formation and distribution
[2000Tze]
HIP, XRD, SEM with EDX and hardness measurements
Formation, characterization and hardness
[2001Lop]
Mill, combustion reaction and XRD
Characterization and phase proportions
[2001Qin]
Arc melting, directional casting, optical microscopy, XRD, SEM, TEM and thermodynamic calculations
Characterization and microstructure stability
[2001Yan]
Mill, press, XRD, optical microscopy SEM and TEM
Formation, characterization and alloy compositions to avoid deleterious TiAl3
[2001Zha]
Arc melting, XRD and SEM with EDX
Formation and characterization
[2002Bar]
Electrical and mechanical properties
Electrical and thermal characterization of Ti2AlC
[2002Gaz]
Metallography, LiMCA and PoDFA
Particle kinetics characteristics
[2002Ge]
Combustion, DSC
Formation kinetics of Ti3AlC2
[2002Kho1]
High energy attrition mill, XRD, SEM with EDS
Formation and characterization
[2002Mei]
SPS, XRD and EPMA
Formation and characterization
[2002Ria]
Arc melting, optical microscopy, Characterization and dendrite SEM, image analysis and XRD arm spacing of TiC
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
15
16
6
Al–C–Ti
. Table 5 (continued) Method / Experimental Technique
Reference
Type of Property
[2002Tro]
Thermoelectric (TEP) measurements, metallography and SEM with EDX
Formation, characterization and effect on grain refining
[2002Wan1, 2002Wan2, 2004Wan1, 2004Wan2, 2006Lee]
Oxidation studies
Synthesis and oxidation of Ti3AlC2
[2002Xia, 2002Liu]
Metallography, SEM
Characterization and distribution of particles; effectiveness of grain refining
[2002Zha1]
Melt spinning, XRD and SEM
Formation and characterization; effect on grain refining
[2002Zha2]
Arc melting, XRD, SEM with EDS, Formation, characterization; nanoindenter microhardness and modulus
[2003Arp]
Pressure infiltration, DTA, XRD and SEM
(Al)/TiC composite manufacture and characterization
[2003Guo1, 2003Guo2, 2004Guo]
Combustion chamber studies
Formation of TiC1–x, Ti3AlC2
[2003Hua]
Reactions of activated Al-Ti-C powder under laser
Formation and characterization
[2003Guo1, 2003Guo3]
Combustion chamber, XRD, SEM Formation and characterization of Ti2AlC1–x
[2003Son, 2004Son2]
Mill, “DERP” thermal analysis furnace, optical microscopy, XRD, SEM with EDS and TEM
Formation and characterization
[2003Sun]
Bulk modulus studies
Ti2AlC bulk modulus
[2003Wan2]
Ball milling, DSC and XRD
Formation reactions for TiC for grain refiners
[2003Zha1]
Melt spinning, XRD, SEM and TEM
Formation and characterization
[2003Zha2]
DTA, XRD, SEM
Formation and characterization
[2003Zho]
SPS, HIP, XRD and SEM
Formation and characterization of Ti3AlC2
[2004Hon, 2005Hon]
Press, XRD, SEM, density and hardness measurements
Characterization, density and hardness
[2004Hwa, 2004Wan3, 2005Wan4]
SHS combustion chamber, XRD and SEM with WLS and EDX
Precipitate characterization, formation and distribution
[2004Kex, 2005Rog]
Ball mill, combustion synthesis reactor, XRD and SEM with EDS
Formation and characterization
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Table 5 (continued) Reference
Method / Experimental Technique
Type of Property
[2004Mei, 2005Zho1, 2005Zho2]
Spark plasma sintering (SPS), XRD and SEM with EDS.
Manufacture, characterization and density of Ti2AlC
[2004Son1]
Mill, hydrostatic press, SEM and TEM with EDS
Formation and characterization of Ti3AlC2
[2001Zho1]
XRD, electronic measurements
Structure and electrical properties of Ti3AlC2
[2005Bao]
Electrical and mechanical properties
Thermal shock of Ti3AlC2
[2005Jia, 2006Xia]
SHS combustion chamber, XRD, Precipitate characterization, DTA and SEM with WLS and EDX formation and distribution
[2005Kho]
SHS combustion chamber, press, Characterization, formation and XRD, SEM with EDX, EPMA and distribution image analysis
[2005Kum]
XRD, SEM with EDX
Characterization of master alloy, and grain-refined alloys
[2005Li]
SHS combustion chamber, XRD, XRF, SEM with EDX and thermodynamic calculations
Precipitate characterization, formation and distribution
[2005Pen]
Press, XRD and SEM
Characterization and density
[2005Wal]
Sputtering chamber, XRD and XPS
Characterization
[2005Wan1, 2005Wan2]
Sintering, pressing, mechanical Manufacture, characterization, tests and XRD, SEM with EDX and three-point bend tests, harnesses density measurements and fracture toughness
[2005Xia]
Al-C-Ti launders and moulds, electromagnetic field
Precipitate characterization and distribution
[2005Zha]
Equal-channel angular press, SEM and microhardness tester
Formation, precipitate characterization and distribution; hardness
[2006Li]
Mechanical alloying, XRD and SEM
Formation and characterization
[2006Sel]
Powder metallurgy, optical Formation, characterization, yield microscopy, SEM and mechanical stress, UTS, ductility and Young’s measurements modulus.
[2006Zho]
Uniaxial compression and indentation by hemispherical nanoindenor
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
Mechanical properties, including bulk modulus and Poisson’s ratio, at different orientations
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
17
18
6
Al–C–Ti
. Fig. 1 Al-C-Ti. Adopted Al-Ti phase diagram
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Fig. 2 Al-C-Ti. Adopted C-Ti phase diagram
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
19
20
6
Al–C–Ti
. Fig. 3 Al-C-Ti. Partial isothermal section at 1250˚C
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Fig. 4 Al-C-Ti. Partial isothermal section at 1050˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
21
22
6
Al–C–Ti
. Fig. 5 Al-C-Ti. Isothermal section at 1000˚C
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Fig. 6 Al-C-Ti. Partial isothermal section at 750˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
23
24
6
Al–C–Ti
. Fig. 7 Al-C-Ti. Isopleth at 2 mass% Al for the concentration range 0–1 mass% C, plotted in at.%
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Fig. 8 Al-C-Ti. Isopleth at 4 mass% Al for the concentration range 0–1 mass% C, plotted in at.%
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
25
26
6
Al–C–Ti
. Fig. 9 Al-C-Ti. Isopleth at 6 mass% Al for the concentration range 0–1 mass% C, plotted in at.%
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Fig. 10 Al-C-Ti. Isopleth at 8 mass% Al for the concentration range 0–1 mass% C, plotted in at.%
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
27
28
6
Al–C–Ti
. Fig. 11 Al-C-Ti. Isopleth at 10 mass% Al for the concentration range 0–1 mass% C, plotted in at.%
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti
6
. Fig. 12 Al-C-Ti. Vertical section γ(TiAl) - TiC1–x
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
29
30
6
Al–C–Ti
References [1949Cib] [1954Thy] [1963Jei] [1964Jei] [1964Now]
[1965Mol]
[1966Yas] [1967Hod]
[1972Cis] [1972Now] [1976Ivc1]
[1976Ivc2]
[1976Jon]
[1977Gur]
[1977Ivc]
[1980Mii] [1980Pea]
[1980Sch]
[1982Bla] [1982Now]
[1982Wit]
Cibula, A., J. Inst. Met., 76, 321 (1949), as quoted in [2000Sch] van Thyne, R.J., Kesler, H.D., “Influence of Oxygen, Nitrogen and Carbon on the Phase Relationships in the Ti-Al System”, Trans. AIME, J. Metals, 193–199 (1954) (Experimental, Phase Diagram, 7) Jeitschko, W., Nowotny, H., Benesovsky, F., “Carbon Containing Ternary Compounds (H-Phase)” (in German), Monatsh. Chem., 94, 672–676 (1963) (Crys. Structure, Experimental, 6) Jeitschko, W., Nowotny, H., Benesovsky, F., “Ti3AlC, A Perowskite-Carbide” (in German), Monatsh. Chemie, 95, 319–321 (1964) (Crys. Structure, Experimental, 4) Nowotny, H., Jeitschko, W., Benesovsky, F., “Novel Complex Carbides and Nitrides and Their Relation to Phases of Hard Substances” (in German), Planseeber. Pulvermet., 12, 31–43 (1964) (Crys. Structure, Experimental, Phase Relations, 18) Molchanova, E.K., “Titanium-Aluminum-Carbon” in “Phase Diagrams of Titanium Alloys”, Glazunov, S.G. (Ed.), Israel Program Scientific Translations, Jerusalem, 256–259 (1965) (Experimental, Phase Diagram, 1) Yasinskaya, G.A., (in Russian), Poroshk. Metall. (Kiev), 43(7), 53–55 (1966) (Experimental, Mechan. Prop., 5) Hodson, R.L., Parikh, N.M., “Cermented Carbides with High-Melting Binders. II. Ternary Equilibrium System”, J. Powder Metall., 3, 31–40 (1967) (Experimental, Mechan. Prop., Morphology, Phase Relations, 6) Cisse, J., Bolling, G.F., Kerr, H.W., J. Crys. Growth, 13/14, 777–781 (1972), as quoted in [1976Jon] Nowotny, H., “Crystallochemistry of Complex Carbides and Related Compounds” (in German), Angew. Chem., 84, 973–982 (1972) (Crys. Structure, Experimental, 71) Ivchenko, V.I., Lesnaya, M.I., Nemchenko, V.F., Kosolapova, T.Ya., “Some Physical Properties of Ternary Compounds in the Ti-Al-C System”, Sov. Powder Metall. Met. Ceram., 367–369 (1976), translated from Poroshk. Metall., 5(161), 45–48 (1976) (Crys. Structure, Electr. Prop., Experimental, Phys. Prop., 11) Ivchenko, V.I., Kosolapova, T.Ya, “Ternary Phases in the Titanium-Aluminium-Carbon System” in “Karbidy Splavy Ikh Osnove”, (in Russian), Samsonov, G.V., Kosolapova, T.Ya., Gnesin, G.G., (Eds.), Naukova Dumka, Kiev, USSR, 54–56 (1976) (Experimental, 5) Jones, G. P., Pearson, J., “Factors Affecting the Grain-Refinement of Aluminum Using Titanium and Boron Additives”, Metall. Trans. B, 7(1), 223–234 (1976) (Assessment, Phase Diagram, Review, Thermodyn., 12) Gurin, V.N., Korsukova, M.M., Popov, V.I., Elizarova, O.V., Belozov, N.N., Kuz’ma, Yu.B., “Solid Solutions of B, C, Si in Aluiminides of Transient Metals” in “Single Crystals of Refractory and Rare Metals, Alloys and Compounds”, (in Russian), Tananaev, I.V. (Ed.), Nauka, Moscow, 39–42 (1977) (Crys. Structure, Experimental, Phase Diagram, 6) Ivchenko, V.I., Kosolapova, T.Y., “Study of Preparation Conditions and Certain Properties of Ternary Compounds in the Ti-Al-C and Ti-Al-N Systems” (in Russian), Nauch. Trudy Moskov. Inst. Stali I Splavov, 99, 86–90 (1977) (Experimental, Kinetics, 11) Miida, R., Kasahara, M., Watanabe, D., Jpn. J. Appl. Phys., 19, L707-L710 (1980), as quoted in [1990Sch] Pearson, W.B., “Dimensional Analysis of Interstitial Phases with the AlCr2C Structure”, Acta Crystallogr., Sect. A: Found. Crystallogr., 36(4), 724–732 (1980) (Crys. Structure, Electronic Structure, Experimental, 11) Schuster, J.C., Nowotny, H., Vaccaro, C., “The Ternary Systems: Cr-Al-C, V-Al-C and Ti-Al-C and the Beahviour of the H-Phases (M2AlC)”, J. Solid State Chem., 32, 213–219 (1980) (Crys. Structure, Experimental, Phase Diagram, 10) Blake, N.W., Ph.D. Thesis, Queens University, ON, Canada, 1982 as quoted in [1993Sve] Nowotny, H., Rogl, P., Schuster, J.C., “Structural Chemistry of Complex Carbides and Related Compounds”, J. Solid State Chem., 44, 126–133 (1982) (Crys. Structure, Experimental, Phase Relations, Review, 33) Wittmer, M., “Interfacial Recations Between Aluminium and Transition-Metal Nitride and Crabide Films”, J. Appl. Phys., 53(2), 1007–1012 (1982) (Crys. Structure, Experimental, Morphology, Phase Relations, 16)
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti [1984Ker]
[1986Ban] [1986Bat]
[1986Mii] [1987Zak]
[1989Cam1] [1989Cam2] [1990Cam] [1990Hay]
[1990Sch] [1990Via]
[1991Cam1]
[1991Cam2]
[1991Fro] [1991Jar]
[1991Kno] [1991Mab]
[1991Rap] [1991Sah] [1991Yok]
[1992Aye] [1992Che] [1992Cho]
6
Kerans, R.J., Mazdiyasni, K.S., Ruh, R., Lipsitt, H.A., “Solubility of Metals in Substoichiometric TiC(1–x)”, J. Am. Ceram. Soc., 67, 34–38 (1984) (Experimental, Mechan. Prop., Morphology, Phase Diagram, Phase Relations, 29) Banerji, A., Reif, W., “Development of Al-Ti-C Grain Refiners Containing TiC”, Metall. Trans. A, 17, 2127–2137 (1986) (Calculation, Experimental, Morphology, Phase Relations, Thermodyn., 28) Baturinskaya, N.L., Kalchuk, N.A., Sezonenko, Yu.D., Chernyi, V.G., “Cast Dispersion-Hardemed Aluminum Alloys with a High Titanium Carbide Content”, Russ. Metall., 3, 145–147 (1986) (Experimental, 3) Miida, R., Jap. J. Appl. Phys., 25, 1815–1824 (1988), as quoted in [1990Sch] Zakharov, A.M., Lashkova, L.A.K; Semeryakova, S.G., “Polythermal Section (γ)TiAl-TiC of the Ti-Al-C System”, Russ. Metall. (Engl. Transl.), (4), 197–198 (1987), translated from Izv. Akad. Nauk SSSR, Met., (4), 196–197 (1987) (Crys. Structure, Experimental, Phase Diagram, 7) Cam, G., Flower, H.M., D. R. F. West, D.R.F., “The Alloying of Titanium Aluminides with Carbon”, Mater. Res. Soc. Symp. Proc., 133, 663–668 (1989) (Experimental, Morphology, Phase Relations, 7) Cam, G., Flower, H.M., West, D.R.F., “Phase Transformations in Ti-Al-C Alloys”, Proc. Euromat ’89, Aachen, 1–6 (1989) (Experimental, Morphology, Phase Relations, 7) Cam, G., Ph.D. Thesis, Imperial College, University of London, 1990, as quoted in [2000Ria] Hayes, F. “Al-C-Ti (Aluminium-Carbon-Titanium)” in MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.14870.1.20, (1998), also published in “Ternary Alloys”, Petzow, G., Effenberg, G. (Eds.), Vol. 3, VCH Verlagsgesellschaft, Weinheim, Germany, 557–566 (1990) (Phase Diagram, Review, 15) Schuster, J.C., Isper, H., “Phases and Phase Relations in the Partial System TiAl3-TiAl”, Z. Metallkd., 81 (6), 389–396 (1990) (Phase Diagram, Experimental, 33) Viala, J.C., Vincent, C., Vincent, H., Bouix, J., “Thermodynamic Approach of the Chemical Interaction between Aluminium and Carbon-Titanium” (in French), Mater. Res. Bull., 25, 457–464 (1990) (Experimental, Phase Diagram, Phase Relations, 20) Cam, G., Flower, H.M., West, D.R.F., “Constitution of Ti-Al-C Alloys in the Temperature Range 1250750˚C”, Mater. Sci. Technol., 7, 505–511 (1991) (Experimental, Morphology, Phase Diagram, Phase Relations, 15) Cam, G., Flower, H.M., West, D.R.F., “Solid State Phase Transformations in Titanium-AluminumCarbon and Titanium-Aluminum-Niobium-Carbon Alloys”, Mater. Sci. Technol., 7(7), 587–591 (1991) (Crys. Structure, Experimental, Morphology, Phase Relations, 10) Froyen, L., Delaey, L., “In Situ Formation of Aluminium Composites”, COST 507 Leuven Proc., Commission of the European Communities, Part A, B1 (1991) (Experimental, 1) Jarfors, A., Fredriksson, H., Froyen, L., “On the Thermodynamics and Kinetiks of Carbides in the Aluminium-rich Corner of the Al-Ti-C Phase Diagram”, Mater. Sci. Eng. A, 135, 119–123 (1991) (Assessment, Experimental, Kinetics, Phase Diagram, Thermodyn., 5) Knotek, O., Lo¨ffler, F., Wolkers, L., “On the Phase Stability and Transition of Metastable TiAlC and TiAlN-PVD-coatings”, COST 507 Leuven Proc., Part A, D7, (1991) (Experimental, 4) Mabuchi, H., Harada, K., Tsuda, H., Nakayama, Y., “Fabrication of Ti2AlC/TiAl Composites Using Combustion Reaction Process”, ISIJ Int., 31(10), 1272–1278 (1991) (Crys. Structure, Experimental, Interface Phenomena, Morphology, Thermodyn., 20) Rapp, R.A., Zheng, X., “Thermodynamic Consideration of Grain Refinement of Aluminium Alloys by Titanium and Carbon”, Metall. Trans. A, 22A, 3071–3075 (1991) (Calculation, Thermodyn., 7) Sahoo, P., Koczak, M.J., “Analysis of in Situ Formation of Titanium Carbide in Aluminum Alloys”, Mater. Sci. Eng. A, 144(1-2), 37–44 (1991) (Experimental, Kinetics, Thermodyn., 23) Yokokawa, H., Sakai, N., Kawada, T., Dokiya, M., “Chemical Potential Diagram of Al-Ti-C System: Al4C3 Formation on TiC Formed in Al-Ti Liquids Containing Carbon”, Metall. Trans. A, 22A, 3075–3076 (1991) (Calculation, Phase Diagram, Thermodyn., 11) Ayer, R., Ray, R., Scanlon, J.C., “Analytical Microscopy of a γ-TiAl Composite Containing a Carbide Phase”, Scr. Metall. Mater., 26(9), 1337–1342 (1992) (Crys. Structure, 19) Chen, S., Beaven, P.A., Wagner, R., “Carbide Precipitation in γ-TiAl Alloys”, Scr. Metall. Mater., 26(8), 1205–1210 (1992) (Electronic Structure, Experimental, Morphology, 10) Choi, Y., Mullins, M.E., Wijayatilleke, K., Lee, J.K., “Fabrication of Metal Matrix Composites of TiC-Al Through Self-Propagating Synthesis Reaction”, Metall. Trans. A, 23(9), 2387–2392, 1992 (Experimental, Morphology, 14)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
31
32
6 [1992Jar]
[1992Pie] [1992Vol]
[1993Ber]
[1993Cho]
[2003Fri] [1993Den]
[1993Jar]
[1993Mit]
[1993Sve] [1993Tia]
[1994Bra] [1994Din] [1994May]
[1994Pie]
[1994Ton]
[1994Whi]
[1994Zha] [1995Mor]
[1995Nuk] [1995Via]
Al–C–Ti Jarfors, A.E.W., Fredriksson, H., “The Reaction Between Titanium Carbide and Aluminum Carbide in Liquid Aluminum; A Microgravity Study”, Eur. Space Agency, ESA SP-333, Proc. VIIIth European Symposium on Materials and Fluid Sciences in Microgravity, Vol. 20, 849–854 (1992) Pietzka, M.A.O., “Structural Chemistry, Phase Equilibria and Chemical Analysin in the Ti-Al-C and Ti-Al-N Systems” (in German), Dipl., Uni. Wien, 1–52 (1992) (Phase Diagram, 35) Vol’ne, B.M., Evstigneev, V.V., “Structure Formation in the SHS-System Titanium Aluminum Carbon”, Combustion Explosion and Shock Waves, 28(2), 173–178 (1992) (Crys. Structure, Experimental, Morphology, 8) Bergman, A., Jarfors, A., Liu, Z., Fredriksson, H., “In-situ Formation of Carbide Composites by Liquid/Solid Reactions”, Key Eng. Mater., 79-80, 213–233 (1993) (Calculation, Experimental, Morphology, Phase Diagram, Phase Relations, 9) Choi, Y., Rhee, S.W., “Effect of Aluminium Addition on the Combustion Reaction of Titanium and Carbon to Form TiC”, J. Mater. Sci., 28(24), 6669–6675 (1993) (Crys. Structure, Experimental, Interface Phenomena, Morphology, Thermodyn., 17) Frisk, K., “A Revised Thermodynamic Description of the Ti-C System”, Calphad, 27(3), 367–373 (2003) (Phase Diagram, Phase Relations, Thermodyn., Assessment, 22) Denauin, A., Naka, S., Huguet, A., Menand, A., “Atom-Probe Investigation of the Partitioning of Interstitial Elements in Two-Phase γ + α2 Ti-Al-Based Alloys”, Scr. Metall. Mater., 28(9), 1131–1136 (1993) (Crys. Structure, Experimental, 8) Jarfors, A.E.W., Svendsen, L., Wallinder, M., Fredriksson, H., “Reactions During Infiltration of Graphite Fibers by Molten Al-Ti Alloy”, Metall. Trans. A, 24A(11), 2577 (1993) (Experimental, Mechan. Prop., Phase Diagram, Thermodyn., 17) Mitra, R., Fine, M.E., Weertman, J.R., “Chemical Reaction Strengthening of Al/TiC Metal Matrix Composites by Isothermal Heat Treatment at 913 K”, J. Mater. Res., 8(9), 2370–2379 (1993) (Crys. Structure, Experimental, Morphology, Phase Relations, Thermodyn., 25) Svendsen, L., Jarfors, A., “Al-Ti-C Phase Diagram”, Mater. Sci. Technol., 9, 948–957 (1993) (Experimental, Phase Diagram, Thermodyn., 17) Tian, W.H., Harada, K., Nakashima, R., Sano, T., Nemoto, M., “Crystal Structures and Morphologies of Carbide and Nitride Precipitates in TiAl” (in Japanese), J. Jpn. Inst. Met., 57(11), 1235–1243 (1993) (Crys. Structure, Experimental, Phase Diagram, 17) Braun, J., Ellner, M., Predel, B., Z. Metallkd., 85, 855–862 (1994) as quoted in [2001Bra] Dinsdale, A., “Summary of the Proceedings of the CALPHAD XXIII-CAMSE 94 Meeting”, Calphad, 18 (4), 337–368 (1994) (Abstract, Calculation, Phase Diagram, 52) Mayes, C.D., McCartney, D.G., Tatlock, G.J., “Observations on the Microstructure and Perfomance of an Al-Ti-C Grain-Refining Master Alloy”, Mater. Sci. Eng. A, 188, 283–290 (1994) (Crys. Structure, Experimental, Morphology, Phase Diagram, Phase Relations, 29) Pietzka, M.A., Schuster, J.C., “Summary of Constitutional Data on the Aluminium-Carbon-Titanium System”, J. Phase Equilib., 15(4), 392–400 (1994) (Calculation, Experimental, Phase Diagram, Phase Relations, Thermodyn., 23) Tong, X., Shen, N., Liu, B., “Formation and Distribution of TiC Phase in Rapidly Quenched Al-3.18Ti-0.65C Alloy” (in Japanese), Acta Metall. Sin., Ser. A, 30(4), 155–159 (1994) (Experimental, Thermodyn., 2) Whittenberger, J.D., Ray, R., Farmer, S.C., “Elevated-Temperature Deformation Properties of In-Situ Carbide Particle Strengthened Ti-48Al Materials”, Intermetallics, 2(3), 167–178 (1994) (Crys. Structure, Experimental, Morphology, Thermodyn., 19) Zhang, M.X., Chang, Y.A., “Phase Diagrams of Ti-Al-C, Ti-Y-O, Nb-Y-O, and Nb-Al-O at 1100˚C”, J. Phase Equilib., 15(5), 470–472 (1994) (Experimental, Phase Diagram, Phase Relations, 12) Morimoto, H., Nomura, M., Ashida, Y., “In-Situ TiC Particulate Reinforced Aluminum Composites Fabricated by Reaction Between Graphite Particles and Liquid Al-Ti Alloys” (in Japanese), J. Jpn. Inst. Met., 4, 429–436 (1995) (Crys. Structure, Experimental, Morphology, Phys. Prop., Thermodyn., 24) Nukami, T., Flemings, M.C., Metall. Mater. Trans., 24A (1995) as quoted in [2000Tjo] Viala, J.C., Peillon, N., Clochefert, L., Bouix, J., “Diffusion Paths and Reaction Mechanisms in the High-Temperature Chemical Interaction Between Carbon and Titanium Aluminides”, Mater. Sci. Eng. A, 203, 222–237 (1995) (Experimental, Interface Phenomena, Kinetics, Phase Diagram, Phase Relations, Thermodyn., 22)
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti [1996Cha] [1996Ily]
[1996Mat] [1996Sob]
[1996Sun] [1996Tom]
[1997Chr] [1997Ich]
[1997Ily1]
[1997Ily2] [1997Li] [1997Lee]
[1997Sah]
[1997Wu] [1997Ye] [1998Fra]
[1998Mat]
[1998Tan]
[1999Abe]
[1999Bir]
6
Chang, W-S., Muddle, B.C., “Precipitation of (Ti,V)2Al(C,N,) in Multiphase Al-Ti-V Alloys”, Mater. Sci. Eng. A, 207, 64–71 (1996) (Crys. Structure, Experimental, 18) Ilyasov, V.V., Nikiforov, I.Ya., Ilyasov, Yu.V., “Electronic Energy Structure of the Ternary Carbide System Ti-Al-C”, Phys. Status Solidi B, 198, 687–693 (1996) (Calculation, Crys. Structure, Mechan. Prop., Phys. Prop., 22) Matar, S.F., Etourneau, J., “Investigation of the Electronic Structure of Carbon-Containing TiAl”, J. Alloys Compd., 233(1-2), 112–120 (1996) (Crys. Structure, Experimental, Thermodyn., 10) Sobczak, N., Gorny, Z., Ksiazek, M., Radziwill, W., Rohatgi, P., “Interaction Between Porous Graphite Substrate and Liquid or Semi-liquid Aluminum Alloys Containing Titanium”, Mater. Sci. Forum, 217-222, 153–158 (1996) (Crys. Structure, Experimental, Morphology, Thermodyn., 17) Sun, X., Mei, B., Yu, A.R., Liao, G., “Thermal Explosion Synthesis in Ti-C-Al System”, Acta Metall. Sin., 32(10), 1102–1106, 1996 (Experimental, Morphology, 3) Tomoshige, R., Matsushita, T., “Production of Titanium-Aluminum-Carbon Ternary Composites with Dispersed Fine TiC Particles by Combustion Synthesis and Their Microstructure Observations” (in Japanese), J. Ceram. Soc. Jpn., 104(2), 94–100 (1996) (Crys. Structure, Experimental, Morphology, Thermodyn., 14) Christoph, U., Appel, F., Wagner, R., “Dislocation Dynamics in Carbon-Doped Titanium Aluminide Alloys”, Mater. Sci. Eng. A, 240, 39–45 (1997) (Experimental, Morphology, Thermodyn., 15) Ichikawa, K., Kinoshita, Y., “Rheocasting Techniques Applied to Intermetallic TiAl Alloys and Composites”, Mater. Sci. Eng. A, 239-240, 493–502 (1997) (Experimental, Mechan. Prop., Phase Relations, 16) Ilyasov, V.V., Nikiforov, I.Ya., “Computer Simulation of the Electronic Structure and Chemical Bond in the Ternary System Ti1–xAlxC”, Phys. Solid State, 39(2), 185–188 (1997) (Calculation, Phys. Prop., 22) Ilyasov, V.V., Nikiforov, I.Ya., Ilyasov, Yu.V., “Ti L-Spectrum XANES and Electron Structure of the System Ti-Al-C”, J. Phys. IV, France, 7(C2), 281–282 (1997) (Experimental, 9) Li, J., Hao, S., “α (α2) and γ Phase Equilibria in Ti-Al-C and Ti-Al-B Ternary Systems”, Trans. Nonferrous Met. Soc. China, 7(2), 63–66 (1997) (Experimental, Morphology, Phase Relations, 10) Lee, W.-C., Chung, S.-L., “Ignition Phenomena and Reaction Mechanisms of the Self-Propagating High-Temperature Synthesis Reaction in the Titanium-Carbon-Aluminum System”, J. Am. Ceram. Soc., 80(1), 53–61 (1997) (Crys. Structure, Experimental, Interface Phenomena, Morphology, Thermodyn., 20) Sahu, P.Ch., Chandra Shekar, N.V., Yousuf, M., Govinda Rajan, K., “Implications of a Pressure Induced Phase Transition in the Search for Cubic Ti3Al”, Phys. Rev. Lett., 78(6), 1054–1057 (1997) (Crys. Structure, Experimental, 20) Wu, N.Q., Wu, J.M., Li, Z.Z., Wang, G.-X., “Formation of Nanocrystalline F.C.C. Phase by Mechanically Driven Crystallization”, Mater. Trans., JIM, 38(3), 255–259 (1997) (Experimental, 16) Ye, L.L., Liu, Z.G., Li, S.D., Quan, M.X., Hu, Z.Q., “Thermochemistry of Combustion Reaction in AlTi-C System During Mechanical Alloying”, J. Mater. Res., 12(3), 616–618 (1997) (Experimental, 19) Frange, N., Frumin, N., Levin, L., Polak, M., Dariel, M.P., “High-Temperature Phase Equilibria in the Al-Rich Corner of the Al-Ti-C System”, Metall. Mater. Trans. A, 29, 1341–1345 (1998) (Calculation, Experimental, Phase Relations, Thermodyn., 27) Matar, S.F., Petitcorps, Y.L., Etourneau, J., “Ab Initio Study of the Chemical Role of Carbon within TiAl Alloy System: Application to Composite Materials”, Comput. Mater. Sci., 10, 314–318 (1998) (Abstract, Experimental, 7) Tanaka, H., Tomoshige, R., Imamura, K., Chiba, A., Kato, A., “Hot-shock Consolidation and Mechanical/thermal Properties of Ti-Al-C Composites Using Explosive Shock Energy and Combustion Synthesis” (in Japanese), J. Ceram. Soc. Jpn., 106(7), 676–681 (1998) (Experimental, Interface Phenomena, Morphology, 17) Abe, E., Ohnuma, M., Nakamura, M. “The Structure of a New ε-Phase Formed During the Early Stage of Crystallization of Ti-48 at.% Al Amorphous Film”, Acta Mater., 47(13), 3607–3616 (1999) (Crys. Structure, Experimental, 25) Birol, Y., “In Situ Processing of TiCp-Al Composites by Reacting Graphite with Al-Ti Melts”, J. Mater. Sci., 34(7), 1653–1657 (1999) (Experimental, Morphology, 19)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
33
34
6 [1999Dum]
[1999Far]
[1999Ho]
[1999Jar] [1999Li] [1999Zha] [2000Ban]
[2000Bar1] [2000Bri1]
[2000Bri2]
[2000Fin]
[2000Ken]
[2000Ohn]
[2000Ria]
[2000Rom] [2000Sch] [2000Tjo]
[2000Tze]
[2000Van]
[2000Zha1]
Al–C–Ti Dumitrescu, L.F.S., Hillert, M., Sundman, B., “A Reassessment of Ti-C-N based on a Critical Review of Available Assessments of Ti-N and Ti-C”, Z. Metallkd., 90(7), 534–541 (1999) (Calculation, Phase Relations, Phase Diagram, Thermodyn., 38) Farber, L., Levin, I., Barsoum, M.W., El-Raghy, T., Tzenov, T., “High-Resolution Transmission Electron Microscopy of some Tin+1Axn Compounds (n=1, 2; A=Al or Si; X=C or N)”, J. Appl. Phys., 86(5), 2540–2543 (1999) (Crys. Structure, Experimental, 23) Ho, J.C., Hamdeh, H.H., Barsoum, M.W., El-Raghy, T., “Low Temperature Heat Capacities of Ti3Al1.1C1.8, Ti4AlN3, and Ti3SiC2”, J. Appl. Phys., 86(7), 3609–3611 (1999) (Experimental, Thermodyn., 15) Jarfors, A.E.W., “Peritectic-like Precipitation of Titanium Carbide in Al-Ti-C Melts at 1373 K”, Mater. Sci. Technol., 15, 481–494 (1999) (Experimental, Phase Relations, Phys. Prop., Theory, Thermodyn., 29) Li, J., Zong, Y., Hao, Sh., “Effects of Alloy Elements (C, B, Fe, Si) on the Ti-Al Binary Phase Diagram”, J. Mater. Sci. Technol., 15(1), 58–62 (1999) (Experimental, Phase Relations, 13) Zhang, E., Zeng, S., Yang, B., Ma, M., “Formation Process of SHS TiC in Al-Ti-C System”, Intl. J. SelfPropagating High-Temperature Synthesis, 8(1), 59–68 (1999) (Experimental, Morphology, 11) Bandayopadhyay, D., Sharma, R.C., Chakraborti, N., “The Ti-Al-C System (Titanium-AluminiumCarbon)”, J. Phase Equilib., 21(2), 195–198 (2000) (Assessment, Crys. Structure, Phase Diagram, Phase Relations, 11) Barsoum, M.W., Ali, M., El-Raghy, T., “Processing and Characterization of Ti2AlC, Ti2AlN and Ti2AlC0.5N0.5”, Metall. Trans. A, 31A, 1857–1865 (2000) (Crys. Structure, Experimental, 36) Brinkman, H.J., Zupanic, F., Duszczyk, J., Katgerman, L., “Production of Al-Ti-C Grain Refiner Alloys by Reactive Synthesis of Elemental Powders: Part I. Reactive Synthesis and Characterization of Alloys”, J. Mater. Res., 15(12), 2620–2627 (2000) (Crys. Structure, Experimental, Morphology, 16) Brinkman, H.J., Zupanic, F., Duszczyk, J., Katgerman, L., “Production of Al-Ti-C Grain Refiner Alloys by Reactive Synthesis of Elemental Powders: Part II. Grain Refining Performance of Alloys and Secondary Processing”, J. Mater. Res., 15(12), 2628–2635 (2000) (Crys. Structure, Experimental, Morphology, Thermodyn., 9) Finkel, P., Barsoum, M.W., El-Rghy, T., “Low Temperature Dependencies of the Elastic Properties of Ti4AlN3, Ti3Al1.1C1.8, anf Ti3SiC2”, J. Appl. Phys., 87(4), 1701–1703 (2000) (Experimental, Mechan. Prop., 22) Kennedy, A.R., Weston, D.P., Jones, M.J., Enel, C., “Reaction in Al-Ti-C Powders and its Relation to the Formation and Stability of TiC in Al at High Temperatures”, Scr. Mater., 42(12), 1187–1192 (2000) (Experimental, Thermodyn., 12) Ohnuma, I., Fujita, Y., Mitsui, H., Ishikawa, K., Kainuma, R., Ishida, K., “Phase Equilibria in the Ti-Al Binary System”, Acta Mater., 48, 3113–3123 (2000) (Calculation, Experimental, Phase Relations, Thermodyn., 37) Riaz, S., Flower, H.M., West, D.R.F., “Phase Relationships Involving TiC and Ti3AlC (P Phase) in Ti-Al-C System”, Mater. Sci. Technol., 16, 984–992 (2000) (Crys. Structure, Experimental, Phase Relations, 16) Romankiewicz, F., “Grain Refinement of Aluminium with AlTi6C0,1” (in German), Z. Metallkd., 91 (10), 822–825 (2000) (Crys. Structure, Experimental, Mechan. Prop., Phase Relations, 7) Schneider, W., “Grain Refinement of Al Wrought Alloys with Newly Developed AlTiC Master Alloy” (in German), Z. Metallkd., 91(10), 800–806 (2000) (Mechan. Prop., Phase Relations, Review, 14) Tjong, S.C., Ma, Z.Y., “Microstructural and Mechanical Characteristics of in Situ Metal Matrix Composites”, Mater. Sci. Eng., 29, 49–113 (2000) (Crys. Structure, Mechan. Prop., Morphology, Review, Thermodyn., 229) Tzenov, N.V., Barsoum, M.W., “Synthesis and Characterization of Ti3AlC2”, J. Am. Ceram. Soc., 83(4), 825–832 (2000) (Crys. Structure, Electr. Prop., Experimental, Magn. Prop., Mechan. Prop., Phys. Prop., 27) Vandyoussefi, M.V., Worth, J., Greer, A.L., “Effect of Instability of TiC Perticles on Grain Refinement of Al and Al-Mg Alloys by Addition of Al-Ti-C Inoculants”, Mater. Sci. Technol., 16, 1121–1128 (2000) (Calculation, Experimental, Phase Relations, 30) Zhang, B.-Q., Fang, H.-S., Li, J.-G., Ma, H.-T., “An Investigation on Microstructures and Refining Performances of Newly Developed Al-Ti-C Grain Refining Master Alloys”, J. Mater. Sci. Lett., 19(16), 1485–1489 (2000) (Crys. Structure, Experimental, 44)
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti [2000Zha2] [2001Bra] [2001Lop]
[2001Qin]
[2001Yan] [2001Zha]
[2001Zho1] [2001Zho2]
[2002Bar]
[2002Fra] [2002Gaz]
[2002Ge]
[2002Hwa]
[2002Kho1] [2002Kho2] [2002Liu]
[2002Mei] [2002Ria]
[2002Tro]
[2002Wan1] [2002Wan2]
6
Zhang, Z., Liu, X., Bian, X., “Thermodynamics and Kinetic of Forming TiC in Al-Ti-C System” (in Japanese), Acta Chim. Sin., 36(10), 1025–1029 (2000) (Experimental, Morphology, 12) Braun, J., Ellner, M., “Phase equilibria Investigations on the Aluminium-Rich Part of the Binary System Ti-Al”, Metall. Mater. Trans. A, 32A, 1037–1047 (2001) (Phase Diagram, Experimental, 34) Lopacinski, M., Puszynski, J., Lis, J., “Synthesis of Ternary Titanium Aluminum Carbides Using Selfpropagating High-temperature Synthesis Technique”, J. Am. Ceram. Soc., 84(12), 3051–3053 (2001) (Experimental, 11) Qin, G.W., Oikawa, K., Sun,Z.M., Sumi, S., Ikeshoji, T., Wang, J.J., Guo, S.W., Hao, S.M., “Discontinuous Coarsening of the Lamellar Structure of γ-TiAl-Based Intermetallic Alloys and its Control”, Metall. Mater. Trans. A, 32, 1927–1938 (2001) (Crys. Structure, Experimental, Kinetics, Phase Relations, Thermodyn., 46) Yang, B., Chen, G.X., Zhang, J.H., “Effect of Ti/C Additions on the Formation of Al3Ti of in Situ TiC/ Al Composites”, Mater. Design, 22(8), 645–650 (2001) (Experimental, Morphology, 22) Zhang, E., Wang, H., Zeng, S., “Microstructure Characteristics of in Situ Carbide Reinforced Titanium Aluminide (Ti3Al) Matrix Composites”, J. Mater. Sci. Lett., 20, 1733–1735 (2001) (Experimental, Interface Phenomena, Morphology, 7) Zhou, Y.C., Wang, X.H., Sun, Z.M., Chen, S.Q., “Electronic and Structural Properties of the Layered Ternary Carbide Ti3AlC2”, J. Mater. Chem., 11, 2335–2339 (2001) (Calculation, Crys. Structure, 29) Zhou, Y., Sun, Zh., Wang, X., Chen, Sh., “Ab Initio Geometry Optimization and Ground State Properties of Layered Ternary Carbides Ti3MC2 (M=Al, Si and Ge)”, J. Phys.: Condens. Matter, 13(44), 10001–10010 (2001) (Calculation, Crys. Structure, Electronic Structure, 17) Barsoum, M.W., Salama, I., El-Raghy, T., Golczewski, J., Porter, W.D., Wang, H., Seifert, H.J., Aldinger, F., “Thermal and Electrical Properties of Nb2AlC, (Ti,Nb)2AlC and Ti2AlC”, Metall. Mater. Trans. A, 33 (9), 2775–2779 (2004) (Experimental, Thermodyn., 28) Fras, E., Wierzbinski, S., Janas, A., Lopez, H.F., “SHSB Processing and Properties of Al/TiC “in-situ” Composites”, Arch. Metall., 46(4), 407–423 2001 (Experimental, Morphology, 23) Gazanion, F., Chen, X.-G., Dupuis, C., “Studies on the Sedimentation and Agglomeration of Al-Ti-B and Al-Ti-C Grain Refiners”, Mater. Sci. Forum, 396-402, 45–52 (2002) (Experimental, Thermodyn., 12) Ge, Z.B., Chen, K.X., Zhou, H.P., Guo, J.M., “Kinetic Process of Combustion Synthesis of Ternary Carbide Ti3AlC2”, Key Eng. Mater., 224-226, 539–544 (2002) (Experimental, Morphology, Thermodyn., 15) Hwang, C.-C., Chung, S.-L., “Combustion Synthesis in the Ti+C/Ti+Al System - Influence of Reactant Composition”, J. Mater. Sci. Lett., 21(6), 447–450 (2002) (Experimental, Phase Relations, Thermodyn., 15) Khoptiar, Y., Gotman, I., “Ti2AlC Ternary Carbide Synthesized by Thermal Explosion”, Mater. Lett., 57 (1), 72–76 (2002) (Crys. Structure, Experimental, Morphology, Phase Relations, 11) Khoptiar, Y., Gotman, I., Gutmanas, E.Y., “SHS of Ti2AlC and Ti3AlC2 Machinable Ceramics”, Intl. J. Self-Propagating High-Temperature Synthesis, 11(4), 335–44, 2002 (Experimental, Morphology, 16) Liu X.F., Wang, Z.Q., Zhang, Z.G., Bian X.F., “The Relationship Between Microstructures and Refining Performances of Al-Ti-C Master Alloys”, Mater. Sci. Eng. A, 332(1-2), 70–74, 2002 (Experimental, Morphology, 13) Mei, B., Miyamoto, Y., “Investigation of TiAl/Ti2AlC Composites Prepared by Spark Plasma Sintering”, Mater. Chem. Phys., 75, 291–295 (2002) (Experimental, Morphology, Phase Relations, 10) Riaz, S., Flower, H.M., West, D.R.F., “Characteristics of TiC Dendrites in as Solidified Ti-Al-C Alloys”, Mater. Sci. Technol., 18(8), 941–943 (2002) (Crys. Structure, Experimental, Morphology, Phase Relations, 7) Tronche, A., Vandyoussefi, M., Greer, A.L., “Instability of TiC Particles in Aluminium Melts Inoculated with an Al-Ti-C Grain Refiner”, Mater. Sci. Technol., 18(10), 1072–1078 (2002) (Experimental, Phase Relations, 32) Wang, X.H., Zhou, Y.C., “Synthesis and Oxidation of Bulk Ti3AlC2”, Key Eng. Mater., 224-226, 785–790 (2002) (Experimental, Interface Phenomena, 12) Wang, X.H., Zhou, Y. C., “Intermediate-Temperature Oxidation Behavior of Ti2AlC in Air”, J. Mater. Res., 17(11), 2974–2981 (2002) (Experimental, Kinetics, 24)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
35
36
6 [2002Xia]
[2002Zha1]
[2002Zha2]
[2003Arp]
[2003Fri] [2003Ge1]
[2003Ge2]
[2003Guo1]
[2003Guo2]
[2003Guo3] [2003Hua]
[2003Son]
[2003Sun]
[2003Wan1]
[2003Wan2]
[2003Yan]
[2003Zha1] [2003Zha2]
[2003Zho]
Al–C–Ti Xiangfa, L., Zhenqing, W., Zuogui, Z., Xiufang, B., “The Relationship Between Microstructures and Refining Performances of Al-Ti-C Master Alloys”, Mater. Sci. Eng. A, 332, 70–74 (2002) (Crys. Structure, Experimental, Morphology, 16) Zhang, Z., Bian, X., Wang, Z., Liu, X., Wang, Y., “Microstructures and Grain Refinement Perfomance of Rapidly Solidified Al-Ti-C Master Alloys”, J. Alloys Compd., 339, 180–188 (2002) (Experimental, Phase Relations, 25) Zhang, E., Zeng, S., Wang, B., “Preparation and Microstructure of In Situ Particle Reinforced Titanium Matrix Alloy”, J. Mater. Proc. Tech., 125-126, 103–109 (2002) (Experimental, Mechan. Prop., Morphology, 12) Arpon, R., Narciso, J., Louis, E., Garcia-Cordovilla, C., “Interfacial Reactions in Al/TiC Particulate Composites Propduced by Pressure Infitration”, Mater. Sci. Technol., 19, 1225–1230 (2003) (Experimental, Interface Phenomena, Phase Relations, Thermodyn., 22) Frisk, K., “A Revised Thermodynamic Description of the Ti-C System”, Calphad, 27(4), 367–373 (2003) (Assessment, Phase Diagram, Phase Relations, Thermodyn., 22) Ge, Z., Chen, K., Guo, J., Zhou, H., Ferreira, J.M.F., “Combustion Sinthesis of Thernary Carbide Ti3AlC2 in Ti-Al-C System”, J. Eur. Ceram. Soc., 23(3), 567–574 (2003) (Experimental, Phase Diagram, 14) Ge, Z.B., Chen, K.X., Guo, J.M., Zhou, H.P., Ning, X.S., “Formation Mechanism of Ternary Carbide Ti3AlC2 by Combustion Synthesis”, J. Inorg. Mater., 18(2), 427–432 (2003) (Experimental, Morphology, 9) Guo, J.M., Chen K.X., Ge, Z.B., Zho, H.P., Ning, X.S., “Effects of TiC Addition on Combustion Synthesis of Ti(2)AlC Powders” (in Chinese), Acta Metall. Sin., 39(3), 315–319 (2003) (Experimental, Morphology, 18) Guo, J.M., Chen, K.X., Ge, Z.B., Liu, G.H., Zhou, H.P., Ning, X.S., “Effects of Carbon Addition on Combustion Synthesis of Ti3AlC2 Powders” (in Chinese), Acta Metall. Sin., 39(4), 409–413 (2003) (Experimental, Morphology, 17) Guo, J., Chen, K., Ge, Z., Zhou, H., Ning, X., “Combustion Synthesis Ternary Carbide Ti2AlC1–x”, Rare Metal Mater. Eng., 32(12), 1029–1032 (2003) (Experimental, Morphology, 19) Huang, Y., Ma, N., Zou, D., Liang G., Su, J., “Chemical Reactions in Activated Al-Ti-C Powder Mixture under Action of Laser Beam”, Rare Metal Mater. Eng., 32(12), 999–1002 (2003) (Experimental, Morphology, 12) Song, I.-H., Kim, D.K., Hahn, Y.-D., Kim, H.-D., “The Effect of a Dilution Agent on the Dipping Exothermic Reaction Process for Fabricating a High-Volume TiC-reinforced Aluminum Composite”, Scr. Mater., 48(4), 413–418 (2003) (Crys. Structure, Experimental, Morphology, Phys. Prop., 12) Sun, Zh., Ahuja, R., Li, S., Schneider, J.M., “Structure and Bulk Modulus of M2AlC (M = Ti, V, and Cr)”, Appl. Phys. Lett., 83(5), 899–901 (2003) (Calculation, Crys. Structure, Electronic Structure, Kinetics, Mechan. Prop., 15) Wang, J.Y., Zhou, Y.C., “First-Principles Study of Equilibrium Properties and Electronic Structure of Ti3Si0.75Al0.25C2 Solid Solution”, J. Phys.: Condens. Matter, 15(35), 5959–5968 (2003) (Calculation, Crys. Structure, Electronic Structure, Thermodyn., 21) Wang, Z., Liu, X., Zhang, J., Bian, X., “Reaction Mechanism in the Ball-Milled Al-Ti-C Powders”, J. Mater. Sci. Lett., 22(20), 1427–1429 (2003) (Crys. Structure, Experimental, Kinetics, Phase Relations, 6) Yang, B., Wang, F., Zhang, J.S., “Microstructural Characterization of in Situ TiC/Al and TiC/Al-20Si5Fe-3Cu-1Mg Composites Prepared by Spray Deposition”, Acta Mater., 51(17), 4977–4989 (2003) (Crys. Structure, Experimental, Interface Phenomena, Kinetics, Morphology, Phase Relations, Thermodyn., 65) Zhang, Z., Bian, X., Wang, Y., Liu, X., Wang, Z., “TEM Observation of a Rapidly Solidified Al-Ti-C Alloy”, J. Alloys Compd., 349, 121–128 (2003) (Crys. Structure, Experimental, 26) Zhang, B.Q., Fang, H.S., Lu, L., Lai, M.O., Ma, H.T., Li, J.G., “Synthesis Mechanism of an Al-Ti-C Grain Refiner Master Alloy Prepared by New Method”, Metall. Mater. Trans. A, 34(8), 1727–1733 (2003) (Experimental, Thermodyn., 19) Zhou, A., Wang, C.-A., Hunag, Y., “Synthesis and Mechanical Properties of Ti3AlC2 by Spark Plasma Sintering”, J. Mater. Sci., 38(14), 3111–3115 (2003) (Experimental, Mechan. Prop., 14)
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti [2004Guo]
[2004Hon]
[2004Hwa]
[2004Kex] [2004Mei]
[2004Per]
[2004Sch]
[2004Son1]
[2004Son2] [2004Wan1]
[2004Wan2]
[2004Wan3]
[2005App] [2005Bao]
[2005Hon]
[2005Jia]
[2005Kho]
[2005Kum]
[2005Li] [2005Ma]
6
Guo, J.M., Chen, K.X., Zhou, H.P., Ning, X.S., “Effects of TiAl3 Addition in Ti-Al-C System on Combustion Synthesis of Ti3AlC2 Powders” (in Chinese), Acta Metall. Sin., 40(1), 109–112 (2004) (Experimental, Morphology, 14) Hong, X., Mei, B., Zhu, J., Zhou, W., “Fabrication of Ti2AlC by Hot Pressing of Ti, TiC, Al and Active Carbon Powder Mixtures”, J. Mater. Sci., 39(5), 1589–1592 (2004) (Crys. Structure, Experimental, Kinetics, Morphology, Phase Relations, 13) Hwang, C.-C., Chung, S.-L., “A Study of Combustion Synthesis Reaction in the Ti+C/Ti+Al System”, J. Mater. Sci., 39(6), 2073–2080 (2004) (Crys. Structure, Experimental, Morphology, Phase Relations, 18) Kexin, C., Junming, G., Renli, F., Ferreira, J.M.F., “Combustion Synthesis Ternary Carbide Ti2AlC1–x Powders”, Mater. Sci. Forum, 445-456, 191–195 (2004) (Experimental, Morphology, Thermodyn., 11) Mei, B., Zhou, W., Zhu, J., Hong, X., “Synthesis of High-Purity Ti2AlC by Spark Plasma Sintering (SPS) of the Elemental Powders”, J. Mater. Sci., 39(4), 1471–1472 (2004) (Crys. Structure, Experimental, Kinetics, Morphology, 7) Perrot, P., “Al - C (Aluminium - Carbon)”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart, Document ID: 20.15738.1.20, (2004) (Phase Relations, Phase Diagram, Assessment, 19) Schmid-Fetzer, R, “Al-Ti (Aluminum-Titanium)”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 20.15634.1.20 (2004) (Phase Diagram, Phase Relations, Review, 85) Song, I.-H., Kim, D.K., Hahn, Y.-D. Kim, H.-D., “Investigation of Ti3AlC2 in the In-Situ TiC-Al Composite Prepared by the Exothermic Reaction Process in Liquid Aluminum”, Mater. Lett., 58(5), 593–597 (2004) (Experimental, Morphology, 14) Song, I.H., Kim, D.K., Hahn, Y.D., Kim, H.D., “Synthesis of In-Situ TiC-Al Composite by Dipping Exothermic Reaction Process”, Met. Mater. Int., 10(3), 301–306 (2004) (Experimental, Morphology, 26) Wang, X.H., Zhou, Y.C., “Oxidation Behavior of TiC-Containing Ti3AlC2 Based Material at 500-900˚C in Air”, Mater. Res. Innovat., 7(6), 381–390 (2004) (Experimental, Interface Phenomena, Kinetics, Phase Relations, 25) Wang, X.H., Zhou, Y.C., “Improvement of Intermediate-Temperature Oxidation Resistance of Ti3AlC2 by Pre-Oxydation at High Temperatures”, Mater. Res. Innovat., 7(4), 205–211 (2004) (Crys. Structure, Experimental, Interface Phenomena, Kinetics, Morphology, Phase Relations, 10) Wang, H.Y., Jiang, Q.C., Li, X.L., Zhao, F., “Effect of Al Content on the Self-Propagating Hightemperature Synthesis Reaction of Al-Ti-C System in Molten Magnesium”, J. Alloys Compd., 366(1-2), L9–L12 (2004) (Crys. Structure, Experimental, Morphology, 13) Appel, F., “An Electron Microscope Study of Mechanical Twinning and Fracture in TiAl Alloys”, Philos. Mag., 85(2-3), 205–231 (2005) (Experimental, Mechan. Prop., Morphology, Phase Relations, 74) Bao, Y.W., Wang, X.H., Zhang, H.B., Zhou, Y.C., “Thermal Shock Behavior of Ti3AlC2 from Between 200 and 1300˚C”, J. Eur. Ceram. Soc., 25(14), 3367–3374 (2005) (Electr. Prop., Experimental, Mechan. Prop., Morphology, Phys. Prop., Thermodyn., 22) Hongxiang, Z., Zhenying, H., Mingxing, A., Yang, Z., Zhili, Z., Shibo, L., “Tribophysical Properties of Polycrystalline Bulk Ti3AlC2”, J. Am. Ceram. Soc., 88(11), 3270–3274 (2005) (Crys. Structure, Experimental, Mechan. Prop., Morphology, 35) Jiang, Q.C., Wang, H.Y., Zhao, Y.G., Li, X.L., “Solid-State Reaction Behavior of Al-Ti-C Powder Mixture Compacts”, Mater. Res. Bull., 40(3), 521–527 (2005) (Crys. Structure, Experimental, Morphology, Phase Relations, 13) Khoptiar, Y., Gotman, I., Gutmanas, E.Y., “Pressure-Assisted Combustion Synthesis of Dense Layered Ti3AlC2 and its Mechanical Properties”, J. Am. Ceram. Soc., 88(1), 28–33 (2005) (Crys. Structure, Experimental, Mechan. Prop., Morphology, Phase Relations, 11) Kumar, G.S.V., Murty, B.S., Chakraborty, M., “Development of Al-Ti-C Grain Refiners and Study of Their Grain Refining Efficiency on Al and Al-7Si Alloy”, J. Alloys Compd., 396(1-2), 143–150 (2005) (Crys. Structure, Experimental, Interface Phenomena, Morphology, 22) Li, P., Kandalova, E.G., Nikitin, V.I., “In Situ Synthesis of Al-TiC in Aluminum Melt”, Mater. Lett., 59(19-20), 2545–2548 (2005) (Experimental, Morphology, Phase Relations, Thermodyn., 18) Ma, M., Liu, R., Zhao, H., Yu, Y., “In-Situ TiCp/Al Composites Prepared by TE/QP Method”, J. Mater. Sci. Technol., 21(5), 652–656 (2005) (Experimental, Morphology, Phys. Prop., 13)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
37
38
6 [2005Pen] [2005Rog]
[2005Wal] [2005Wan1]
[2005Wan2]
[2005Wan3] [2005Wan4] [2005Xia]
[2005Zha]
[2005Zho1]
[2005Zho2]
[2006Dru]
[2006Lee]
[2006Li]
[2006Lin]
[2006Rag] [2006Sch]
[2006Sel]
[2006Ton]
[2006Xia]
Al–C–Ti Peng, C., Wang, C.-A., Huang, Y., “Synthesis of High Purity Ti3AlC2 Bulk Material by Hot-Pressing”, Key Eng. Mater., 280-283, 1369–1372 (2005) (Experimental, Morphology, 7) Rogachev, A.S., Gachon, J.-C., Grigoryan, H.E., Vrel, D., Schuster, J.C., Sachkova, N.V., “Phase Evolution in the Ti-Al-B and Ti-Al-C Systems During Combustion Synthesis: Time Resolved Study by Synchrotron Radiation Diffraction Analysis”, J. Mater. Sci., 40(9-10), 2689–2691 (2005) (Crys. Structure, Experimental, Phase Relations, 7) Walter, C., Martinez, C., El-Raghy, T., Schneider, J.M., “Towards Large Area MAX Phase Coatings on Steel”, Steel Res., 76(2-3), 225–228 (2005) (Phase Relations, Phys. Prop., Review, 14) Wang, C.-A., Zhou, A., Peng, C., Huang, Y., “Fabrication and Properties of Ti3AlC2-Based Ceramics by Two-Step Method”, Key Eng. Mater., 280-283, 1365–1368 (2005) (Experimental, Mechan. Prop., Phase Relations, 6) Wang, H.Y., Zhao, F., Jiang, Q.C., Wang, Y., Ma, B.X., “Effect of Mg Addition on the Self-Propagating High Temperature Synthesis Reaction in Al-Ti-C System”, J. Mater. Sci., 40(5), 1255–1257 (2005) (Crys. Structure, Experimental, Morphology, Phase Relations, 12) Wang, Ch.-A., Zhou, A., Qi, L., Huang, Y., “Quantitative Phase Analysis in the Ti-Al-C Ternary System by X-ray Diffraction”, Powder Diffr., 20(3), 218–223 (2005) (Experimental, 10) Wang, H., Xia, T., Zhao, W., Liu T., “Preparation of Al-Ti-C Master Alloy by SHS”, Rare Met. Mater. Eng., 34(12), 2009-12, 2005 (Experimental, Morphology, 13) Xiangfa, L., Lina, Y., Jianwen, L., Zhenqing, W., Xiangfa, B., “A New Technique to Refine Pure Aluminum by Al-Ti-C Mold”, Mater. Sci. Eng. A, 399, 267–270 (2005) (Experimental, Interface Phenomena, 13) Zhang, Z., Watanabe, Y., Kim, I., Liu, X., Bian, X., “Microstructure and Refining Performance of an Al-5Ti-0.25C Refiner before and after Equal-Channel Angular Pressing”, Metall. Mater. Trans. A., Suppl., 36A(3), 837–844 (2005) (Experimental, Morphology, 30) Zhou, W.B., Mei, B.C., Zhu, J.Q., Hong, X.L., “Rapid Synthesis of Ti2AlC by Spark Plasma Sintering Technique”, Mater. Lett., 59(1), 131–134 (2005) (Crys. Structure, Experimental, Mechan. Prop., Phys. Prop., 15) Zhou, W., Mei, B., Zhu, J., Hong, X., “Synthesis of High-Purity Ti3SiC2 and Ti3AlC2 by Spark Plasma Sintering (SPS) Technique”, J. Mater. Sci., 40(8), 2099–2100 (2005) (Crys. Structure, Morphology, Experimental, Phys. Prop., 5) Drulis, M.K., Drulis, H., Gupta, S., Barsoum, M.W., El-Raghy, T., “On the Heat Capacities of M2AlC (M=Ti, V, Cr) Ternary Carbides”, J. Appl. Phys., 99(9), 093502 (2006) (Crys. Structure, Electronic Structure, Experimental, Phys. Prop., Thermodyn., 34) Lee, D.B., Park, S.W., “High-temperature Oxidation of Ti3AlC2 Between 1173 and 1473 K in Air”, Mater. Sci. Eng. A, 434(1-2), 147–154 (2006) (Crys. Structure, Experimental, Interface Phenomena, Morphology, Phase Relations, Thermodyn., 15) Li, S.-B., Zhai, H.-X., Bei, G.P., Zhou, Y., Zhang, Z.L., “Formation of Ti3AlC2 by Mechanically Induced Self-Propagating Reaction in Ti-Al-C System at Room Temperature”, Mater. Sci. Technol., 22(6), 667–672 (2006) (Crys. Structure, Experimental, Morphology, 27) Lin, Z.J., Zhuo, M.J., Zhou, Y.C., Li, M.S., Wang, J.Y., “Microstructural Characterization of Layered Ternary Ti2AlC”, Acta Mater., 54(4), 1009–1015 (2006) (Crys. Structure, Experimental, Morphology, 33) Raghavan, V., “Al-C-Ti (Aluminum-Carbon-Titanium)”, J. Phase Equilib. Diffus., 27(2), 148–149 (2006) (Crys. Structure, Phase Diagram, Phase Relations, Review, 14) Schuster, J.C., Palm, M., “Reassessment of the Binary Aluminum-Titanium Phase Diagram”, J. Phase Equilib. Diffus., 27(3), 255–277 (2006) (Assessment, Calculation, Crys. Structure, Phase Diagram, Phase Relations, Thermodyn., 272) Seleuk, C., Kennedy, A.R., “Al-TiC Composite Made by the Addition of Master Alloys Pellets Synthesised from Reacted Elemental Powders”, Mater. Lett., 60(28), 3364–3366 (2006) (Crys. Structure, Experimental, Morphology, 15) Tong, L., Reddy, R.G., “In-Situ Synthesis of TiC-Al (Ti) Nanocomposite Powders by Thermal Plasma Technology”, Metall. Mater. Trans. B, 37B, 531–539 (2006) (Calculation, Crys. Structure, Experimental, Morphology, Thermodyn., 23) Xiao, G.Q., Fan, Q.C., Gu, M.Z., Jin, Z.H., “Microstructural Evolution During the Combustion Synthesis of TiC-Al Cermet with Larger Metallic Particles”, Mater. Sci. Eng. A, 425(1-2), 318–325 (2006) (Crys. Structure, Experimental, Morphology, 33)
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–C–Ti [2006Zho]
[2007Wit]
[Mas2] [V-C2]
6
Zhou, A.G., Barsoum, M.W., Basu, S., Kalidindi, S.R., El-Raghy, T., “Incipient and Regular Kink Bands in Fully Dense and 10 vol.% Porous Ti2AlC”, Acta Mater., 54(6), 1631–1639 (2006) (Experimental, Mechan. Prop., Morphology, 23) Witusiewicz, V.T., Bondar, A.A., Hecht, U., Rex, S., Velikanova, T.Ya., “The Al-B-Nb-Ti System. III. Thermodynamic Re-Evaluation of the Constituent Binary System Al-Ti”, in press, J. Alloys Compd., doi:10.1016/j.jallcom.2007.10.061 (2007) (Phase Relations, Phase Diagram, Experimental, Thermodyn., Calculation, Review, 89) Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_6 ß Springer 2009
39
Al–Cr–Ti
7
Aluminium – Chromium – Titanium Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Natalia Bochvar, Tatiana Dobatkina, Ol’ga Fabrichnaya, Volodymyr Ivanchenko, Damian M. Cupid
Introduction Aluminum and chromium are well known alloying elements used in titanium industry to produce Ti-based alloys [1956Zwi, 1974Zwi, 1990Lam]. Titanium aluminides based on α2 (Ti3Al), γ (TiAl) and TiAl3 are currently being considered as candidate materials for elevated temperature applications as a result of their low density, good corrosion resistance, modulus and attractive high temperature properties [1989Kim, 1991Dur, 1991Moh, 1994Gao, 1995Whi, 1996Liu, 2000Wel, 2000Yan, 2003Zha, 2004Wan, 2005App]. However, these alloys are brittle at temperatures lower than 400 K [2005App]. Alloying with Cr raises their plasticity and resistance to high temperature oxidation [1991Par]. Reviews of experimental studies in the Al-Cr-Ti system were performed by [1953Han, 1992Hay, 2005Rag]. Review of experimental studies up to 1990 is presented by [1992Hay]. Phase equilibria in the Ti rich corner were extensively investigated by [1953Tay, 1958Kor, 1958Tag, 1960Enc]. Partial isothermal sections presented by [1992Hay] in the Ti rich corner and in the range of 600–1200˚C are mainly based on the results of experimental studies of [1960Enc]. [2005Rag] reviewed more recent experimental studies on phase equilibria [2001Fuj, 2000Kai1, 1996Jew1, 1996Jew2, 1996Jew3, 1994Sok]. In the review of [2005Rag], a schematic liquidus surface based on studies of [1997Mab2] and [2001Ich], a reaction scheme and isothermal sections between 497–1200˚C in more extended composition ranges than in [1992Hay] are presented. The Calphad method was used in works [1988Gro, 1999Sha, 2001Kau] to establish a thermodynamic database and to calculate phase diagrams. However, the details of modeling were not reported in these works. The only experimental data for thermodynamic values were obtained by [1999Jac] by vapour pressure measurements. Experimental and theoretical studies of the Al-Cr-Ti system are summarized in Table 1.
Binary Systems The binary diagrams were taken from [2008Cor] for the Al-Cr, from [2007Wit] for the Al-Ti and from [2000Zhu] for the Cr-Ti. The lattice parameters for the binary Al-Ti compounds were taken from [2006Sch] and for the binary Cr-Ti compounds from [2008Iva].
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
1
2
7
Al–Cr–Ti
Solid Phases Three ternary phases exist in the Al-Cr-Ti system. A ternary phase with the ordered structure L12, denoted τ1, was formed by stabilisation of the binary metastable TiAl3(m) compound by Cr addition [1992Nic, 1993Nak, 1994Kla, 1997Par, 2005Rag]. The τ1 phase exhibits a homogeneity range and dissolves from 7 to 15 at.% Cr at 1200˚C, whereas the content of Ti changes from 23 to 27 at.% [1992Nic, 2001Kau]. According to experimental studies of [1997Mab1, 1997Mab2, 2001Ich, 2003Bar] and calculation of Al-Cr-Ti liquidus surface by [1999Sha] phase τ1 most probably forms by a peritectic reaction. The temperature of τ1 formation was about 1350˚C according to [2001Ich]. In the review of [2005Rag] formation of τ1 by peritectic reaction at 1370˚C was postulated. The ternary phase Ti(Cr,Al)2, (C14 ordered phase), denoted τ2, forms in the Al-Cr-Ti system in the solid state by Al substitution of Cr atoms in the structure of the hightemperature γTiCr2 phase. However, according to the available experimental data, τ2 and γTiCr2 never form a single phase (continuous solid solution). Therefore, τ2 and γTiCr2 are considered here as different phases in spite of having the same structure. The high temperature limit of formation of the τ2 phase was not determined exactly. According to [2001Fuj] and [1997Xu], the maximum temperature of stability of τ2 is between 1200 and 1050˚C. The τ2 phase is stable down to room temperature [1978Jac, 1992Nic, 1993Nak, 1994Kla, 1997Par, 1997Mab1, 1997Mab2]. The τ2 phase has a narrow homogeneity range which extends along the Al-Cr side. The Al content in this phase varies from 3 to 20 at.% at 1050˚C [1997Xu], from 5 to 42 at.% at 1000˚C [1996Jew1, 1997Jew] or from 5 to 40 at.% at 800˚C [1996Jew1, 1997Jew]. Deviation of the Ti content from stoichiometric content (33.3 at.% Ti) was insignificant: 1 at.% at 5 at.% Al and 3 at.% at 35 at.% Al at 1000˚C and 3 at.% at 40 at.% Al at 800˚C [1996Jew1, 1997Jew]. It should be mentioned that with an increase in temperature from 1000 to 1050˚C the τ2 phase shrinks due to the extension of the β phase. The ternary phase denoted τ3 based on the ordered B2 phase (β0), forms in the Al-Cr-Ti system in the solid state. The temperature of formation of the τ3 phase was not determined. One can assume that the high temperature stability limit of the τ3 phase is between 1050˚C, where the phase does not exist [1997Xu], and 1000˚C where it was indicated by [1997Jew, 2000Kai1, 2000Kai2]. The τ3 phase is stable down to room temperature [1992Zhe, 1994Zha, 1999Sha, 2001Sun]. It has a large homogeneity range at 1000˚C, which reduces as temperature decreases [1996Jew1, 1997Jew]. This phase was also indicated by [1964Ram, 1964Sch]. It should be mentioned that the τ3 phase has the same structure as the ordered B2 phase (β0) stable in the Al-Ti binary system in the temperature range of 1159–1427˚C. However, these phases are considered as different phases because they never form a continuous solid solution. According to [1997Jew], the TiAl, Ti3Al, and TiAl2 binary phases extend into the ternary system. The αTiCr2 and βTiCr2 phases also extended into the ternary system dissolving 1 and 4 at.% Al, respectively [1996Jew1, 1997Xu]. At 1000˚C, the solubility of Cr in the TiAl phase increased from about 2 at.% to about 8 at. % while the Al content varied from about 47 at.% to 58 at.%. At 800˚C, the maximum solubility of Cr in TiAl was about 4.5 at.% and remained fairly constant within the Al composition range. The solubility of Cr in the Ti3Al phase is about 2.5 at.% in the temperature range from 800 to 1000˚C. The solubility of Cr in TiAl2 phase is 3.5 at.% at 1000˚C and about 6 at.% at 800˚C [1997Jew]. The solubility of Cr in TiAl3(l) is 4 at.% at 497˚C [1994Sok]. DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
The solubility of Ti in the Cr5Al8 phase is about 10 at.% at room temperature [1992Nic, 1993Nak, 1997Mab1]. The binary CrAl7 phase dissolves up to 1.03 at.% Ti according to [1960Zol] or 2 at.% Ti according to [1994Sok]. The crystal structure data of solid phases in the Al-Cr-Ti system are presented in Table 2.
Invariant Equilibria No temperatures or compositions for invariant reactions with liquid have been reported for the Al-Cr-Ti system. The methods of alloy preparation, the experimental technique and phase range studied are presented in Table 1. [2003Bar] experimentally established two univariant eutectic equilibria. The eutectic transformations L Ð τ1 + β and L Ð τ1 + Cr5Al8 are observed in the temperature range 1285–1255˚C and 1260–1225˚C, respectively. Investigating solid state phase equilibria at temperatures of 1000 and 800˚C, [1996Jew1, 1996Jew2] assumed the existence of invariant reactions τ2 + τ1 Ð β + TiAl2, TiAl + τ1 Ð τ2 + TiAl2 and β + Cr5Al8 Ð Cr2Al + τ1 at a temperature of around 890˚C. [1997Jew] assumed one more invariant reaction β + τ3 Ð τ2 + TiAl at a temperature of 1100±10˚C. For this reaction to occur two three-phase reactions should exist. One of them, τ2 Ð τ3 + β was established by [1996Jew1] at approximately 1120˚C and an Al content of 25 at.%. Existence of the other reaction τ3 Ð β + TiAl has not been confirmed. A reaction scheme was suggested in the present evaluation based on the configuration of the liquidus surface from the thermodynamic calculations of [1999Sha], as well as taking into account the nature and positions of the various threephase equilibria presented in the isothermal sections of [1997Jew]. The reaction scheme is shown in Fig. 1. The invariant three-phase reaction (βTi) Ð αTiCr2 +Ti3Al suggested by [1992Hay] was introduced into the reaction scheme. The temperatures of the invariant reactions indicated in the reaction scheme [1992Hay] were not established experimentally, but were evaluated based on the binary phase diagrams and isothermal sections.
Liquidus, Solidus and Solvus Surfaces Liquidus isotherms in the Ti rich corner (50–100 mass% Ti) were presented by [1958Kor] based on DTA results. Liquidus and solidus isotherms for τ1 and a partial liquidus surface showing equilibria between τ1 and the surrounding phases were constructed by [2001Ich] based on experimental studies. However, the Cr2Al and τ2 phases shown on the liquidus surface of [2001Ich] are not expected to be in equilibrium with liquid [2005Rag]. The boundaries of the liquidus surface projection presented in Fig. 2 are accepted according to [1999Sha]. Solid lines show boundaries of phase fields obtained by thermodynamic calculations, while dashed lines indicate the results of experiments carried out for three alloys Ti40Al-10Cr, Ti-50Al-10Cr, Ti-52Al-20Cr (at.%) (their compositions are shown by filled circles [1999Sha]). A part of the univariant reaction L Ð τ1 + β, between two empty circles in Fig. 2 is based on experimental data of [2003Bar] being in agreement with [1999Sha]. The positions of the invariant reactions in the binary Al-Ti and Al-Cr systems were corrected to be in agreement with binary diagrams of Al-Ti [2007Wit] and Al-Cr [2008Cor] accepted in the present evaluation. Additionally, phase equilibria were added in the Al rich corner, near the Al-Cr side. Isotherms at 1350, 1300, and 1250˚C in the primary crystallisation field of the τ1 phase are presented according to experimental data of [2001Ich]. Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
3
4
7
Al–Cr–Ti
[2005Rag] included a primary crystallisation field of the Ti1–xAl1+x solid solution in the liquidus surface. This phase is not considered in the Al-Ti binary system accepted in the present evaluation according to [2007Wit]. Therefore, the Ti1–xAl1+x phase is not shown in Fig. 2 and there are no reactions involving Ti1–xAl1+x in the reaction scheme (Fig. 1). Also, the difference in the liquidis surface of [2005Rag] and the one presented here is that the primary crystallization field of Ti2Al5 (the same as Ti5Al11) in [2005Rag] is much wider and there is an univariant reaction between liquid, Ti5Al11 and bcc (β) phases, while in the present evaluation, such reaction does not occur. The other difference between the present work and [2005Rag] is in the formation of τ1 by a peritectic reaction: [2005Rag] postulated the formation of τ1 from L+Ti5Al11+β, while here we accept its formation from L+TiAl+Ti2Al5 based on the calculations of [1999Sha]. The liquidus presented here is in a good agreement with the liquidus isotherms for τ1 obtained by [2001Ich], while the isotherm at 1350˚C [2001Ich] is outside the primary crystallisation field of the τ1 phase of [2005Rag]. It should be stressed that experimental information about liquidus in the Al-Cr-Ti system is very limited and the liquidus surface presented by [2005Rag] is rather tentative.
Isothermal Sections Phase equilibria investigations in the Al-Cr-Ti system were performed in the following works at various temperatures: [2000Kai2] at 1300˚C, [1992Hay, 1992Nic, 1992Zhe, 1994Kla, 1998Has, 2000Kai2, 2001Fuj] at 1200˚C, [1993Nak, 1997Mab1, 1997Mab2, 1997Par] at 1150˚C, [1992Hay] at 1100˚C, [1997Xu] at 1050˚C, [1991Mab, 1992Hay, 1993Nak, 1993Hao, 1995Bra, 1995Jew, 1995Hao, 1996Jew1, 1996Jew2, 1997Jew, 2000Kai2, 2001Fuj, 2003Nis1] at 1000˚C, [1974Zwi] at 980˚C, [1988Gro, 1992Hay, 1995Bra, 1995Jew, 1996Jew1, 1996Jew2, 1997Jew] at 800˚C, [1974Zwi] at 760˚C, [1992Hay] at 600˚C and [1994Sok] at 497˚ C. Methods of melting, conditions of homogenization followed by thermal treatment are given in Table 1. [1974Zwi] constructed a phase diagram in the Ti rich region, however, the Ti3Al phase was not considered and therefore these equilibria are not very probable. The isothermal section at 497˚C constructed by [1994Sok] is not exactly correct because the binary Cr2Al11 compound shown in this section decomposes at 785˚C according to accepted binary system [2008Cor]. The samples investigated in the works of [1991Mab, 1992Nic, 1992Zhe, 1993Nak, 1994Kla, 1997Mab1, 1997Mab2, 1997Par, 2003Nis1] were not quenched in water after heat treatment, but were furnace cooled or cooled in air. Using furnace or air cooling methods, the equilibrium phases at high temperature are probably not retained at room temperature. Therefore it can be assumed that phase equilibria established in these works belong to temperatures closer to room temperature. A partial isothermal section in the middle part of the system at 1300˚C is presented in Fig. 3 according to [2000Kai2]. Tie lines show equilibria between (αTi) and β, (αTi) and TiAl, and β and TiAl phases, respectively. A partial isothermal section in the Al rich corner at 1200˚C is presented in Fig. 4 according to [2001Fuj]. [2001Fuj] confirmed the existence of the three-phase field β + TiAl + (αTi), indicated by [1992Hay, 1998Has, 2000Kai2]. An isothermal section at 1050˚C constructed by the diffusion couple method [1997Xu] is presented in Fig. 5. The boundary of the β to τ3 transition is constructed according to the DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
data of [2000Kai1]. It should be mentioned that the phase interactions at 1050˚C (Fig. 5) and 1000˚C (Fig. 6) are different. As temperature decreases from 1050˚C, the single-phase β region contracts, whereas τ2 becomes increasingly stable. At 1050˚C, both the τ1 + τ2 two-phase field and the τ3 single-phase field are absent but are present at 1000˚C. Isothermal sections at 1000 and 800˚C are presented in Figs. 6 and 7 according to [1997Jew]. [1997Jew] used results obtained by [1995Jew, 1996Jew1], which studied equilibria adjacent to the Cr-Ti side with the Al content changing between 30 and 60 at.%, and the Al rich region up to 40 at.% Ti and 80 at.% Cr investigated by [1996Jew2]. In these studies, two three-phase fields in the Al-corner were reliably established: Cr2Al + Cr5Al8 + τ1 and TiAl3 + Cr5Al8 + τ1. Other fields were shown by dashed lines and need additional investigations. The boundary between β and τ3 stability fields is shown according to [2000Kai1]. Results of [1997Jew] at 1000˚C are in general agreement with [1993Hao, 1995Hao], who studied Ti rich region of the system by the diffusion couple method. However, the authors of [1993Hao, 1995Hao] did not indicate the existence of the ternary phase τ3 having the B2 structure. Threephase equilibria τ3 + τ2 + TiAl and τ1 + τ2 + TiAl established by [1997Jew] at 1000˚C were confirmed by [2001Fuj], and the Ti3Al + TiAl + τ3 equilibrium was confirmed by [2000Kai2, 2001Fuj]. The isothermal section at 800˚C was corrected to be consistent with the accepted binary systems Cr-Ti [2000Zhu] and Al-Ti [2007Wit]. According to the accepted binary diagrams, the βTiCr2 and Ti2Al5 compounds decompose by eutectoid reactions at temperatures of 804 and 990˚C respectively and therefore should be absent at 800˚C. Results of [1997Jew] are in partial agreement with the Ti rich corner of the isothermal section at 800˚C calculated by [1988Gro], particularly in the existence of the three-phase field αTi + β + Ti3Al. However [1988Gro] did not indicate the existence of the ternary compound τ3 in contrast with [1997Jew]. Phase compositions of the Al-30at.% Ti-15 at.% Cr alloy heat treated in air at 1000˚C and 800˚C for 100 h and cooled in air for 5minutes were studied by [1995Bra]. It was concluded that the τ1 phase is stable at 1000˚C, but decomposes at 800˚C (this was not confirmed in later studies of [1995Jew, 1996Jew1, 1996Jew2, 1997Jew]). A partial isothermal section at 600˚C in the Ti rich region is presented in Fig. 8 according to [1992Hay]. [2001Kau] calculated isothermal sections at 1500, 1300, 1200 and 1000˚C. The melting temperature of the τ1 phase was also calculated at 1284˚C. The calculated isothermal sections are in general agreement with the experimental studies. The differences concern the temperature of formation of the ternary phases τ1 and τ2. According to [2003Bar] and [2003Mor], the melting temperature of τ1 should be above 1284˚C and according to [2001Fuj], the temperature of formation of τ2 should be below 1200˚C.
Temperature – Composition Sections A partial vertical section at the constant content of Cr (5 mass%) was presented by [1953Bus] based on microstructural investigations. [1958Tag] constructed partial vertical sections at Cr/ Al=1, at constant Cr content (3 at.%) and at constant Ti content (83 at.%) based on equilibrium studies of Ti rich alloys. These sections are not shown in the present evaluation because the Al-Ti binary diagram was not known in details at the time and the TiAl3 phase was not detected in [1958Tag]. Vertical sections from Al-25Ti (at.%) to Cr between 6 and 28 at.% Cr were constructed in the works of [1997Mab1, 1997Mab2, 2001Ich] based on the results of Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
5
6
7
Al–Cr–Ti
DTA investigations and microstuctural analysis of alloys quenched from temperatures of 1300, 1250, 1150 and 1000˚C. In the present work, the vertical section at Ti content of 25 at.% is however not presented as it is in contradiction to the liquidus surface and reaction scheme. According to the present evaluation, the τ2 phase does not appear in the liquidus, while equilibria between liquid and τ2 are shown in the vertical section at 25 at.% Ti. [2001Kau] calculated a vertical section from Al to the composition of Ti-50Cr (at.%). However [2001Kau] did not take into account the existence of the ternary phase τ3 and did not distinguish the two phases with the C14 structure: the binary phase γTiCr2 and the ternary phase τ2.
Thermodynamics Al and Ti activity of Al-Cr-Ti alloys were calculated by [1999Jac] from vapour pressure measurements in the range of 950–1400˚C in two two-phase regions (Ti3Al+TiAl and TiAl +τ2). The results are presented in Figs. 9 and 10. Calculations based on the Calphad method were published by [1988Gro], [1999Sha] and [2001Kau]. [1988Gro] presented a calculated partial isothermal section in the Ti rich composition area at 800˚C. In the calculations of [1999Sha] and [2001Kau], ordering in the τ3 phase was not taken into account and the γTiCr2 and τ2 Laves phases were not distinguished. Details of phase modelling were not reported in these papers. [1999Sha] calculated the isothermal section at 1000˚C and the liquidus surface. Kaufman [2001Kau] calculated isothermal sections in the range of 1000–1500˚C and a phase fraction diagram for the Al15Cr4Ti7 composition which is close to the composition of the τ1 phase. According to the calculations of [2001Kau], the τ1 phase melted in a narrow temperature range at around 1284˚C.
Notes on Materials Properties and Applications The addition of Cr to binary titanium aluminides, in particular TiAl and TiAl3, has proven beneficial to properties. Specifically, when Cr was substituted up to 3 at.% Al in TiAl, the yield stress and fracture strain in bending increased, with the increase attributed to solid solution strengthening [1991Hua, 1991Mas, 1993Has, 1993Kaw, 1994Li, 2001Sun]. Cr also stabilizes the cubic phase, nominally Ti25Cr8Al67 when substituted for Al in TiAl3. This cubic phase has much greater compressive and bending fracture strains than the tetragonal TiAl3 phase [1990Mab, 1990Zha, 1991Mik, 1993Nak, 1993Wri, 2001Mil, 2001Yam, 2002Bra]. This cubic phase also has improved oxidation resistance over TiAl3 at 1200˚C, with Cr promoting the formation of a pure Al2O3 scale while suppressing the formation of TiO2 [1991Par]. However, this attempt at overcoming the brittleness of TiAl3 at ambient temperature results in a relatively poor creep strength at high temperatures. Therefore, the methods of mechanical alloying and high energy ball milling were used to prepare the ternary (Al,Cr)3Ti L12intermetallic compound additionally strengthened by small volume fractions of incoherent Y2O3 dispersoids [1997Hei, 2001Sur]. Specifically, at room temperature oxide dispersion strengthening with 3 vol.% Y2O3 increases the Vickers hardness level by about 500 units compared to 200 for the single-phase Ti25Cr8Al67 compound and retained it up to 500˚C on the level of 480 HV. A successful introduction of the material into the industrial scale depends particularly on its room temperature ductility and the efficiency of the chosen production DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
process. [2000Mab] tried to raise the plasticity and yield stress of (Al,Cr)3Ti L12-intermetallic compound by alloying with V. The Vickers hardness increases slightly by the addition of vanadium, and is nearly independent on the Cr+V contents, although the higher titanium alloys have larger hardeness. The bend ductility at ambient temperature is not improved by the addition of vanadium. The best ductility is about 0.5% (plastic bend strain) for the Al-25Ti12Cr-3V alloy. [2003Bar] shows that the transition from single-phase L12 alloys to eutectic L12+β(Cr) microstructures is accompanied by enhancement of both strength and plasticity, while retaining a high elastic modulus. The primary creep strains of various TiAl alloys reported in the literature were analyzed through modeling by [2003Zha]. [2002Cal] showed, that mechanical alloying followed by spark plasma sintering can be used to produce satisfactory materials in the TiAl-Cr and Al3Ti-Cr systems. Remarkably high flow stresses were found. Such strengths have the same order of magnitude as extrapolated values on the basis of the HP slope ky for single phase materials. Deformation mechanisms based on dislocation activity are most likely dominating in the case of TiAl-X alloys. The fracture stresses for nanocrystalline TiAl3-Cr are very high and within an order of magnitude of the theoretical shear strength of Ti. Deformation of microcrystalline TiAl3-Cr produces yield stresses above 1 GPa and some ductility in compression. Intermetallic Ti-63Al-7Cr coatings can be used for protection from high temperature oxidation of Ti based as well as γ-TiAl based alloys [1997Ley]. [2003Lee] reported that Al21Ti-15Cr alloy would be the most effective among many potential L12-based alloys as a suitable coating material for TiAl alloy because the phase stability of this alloy. This result is similar to one published by [2006Fox], who reported that the best oxidation stability at 750–1100˚C is exhibited by the Ti25 Cr20Al55 alloy containing near 70–75 at.% of L12 and 25–30% Laves phases. Further improvement of this alloy’s oxidation stability results from synergistic doping by a small amount (0.1–0.2 at.%) of active metals such as Hf and Yas well as Si (above 1%). [2003Nis1, 2003Nis2] proposed three layer coatings formed by two-step Cr and Al diffusion for TiAl based alloys. [2001Zho] studied the TiAl based coatings with high Cr content. It was shown that they exhibited excellent oxidation resistance at temperatures ranging from 900 to 1000˚C. Excellent oxidation resistance can be attributed to formation of protective alumina on the coatings. Oxide formed on the surface of Ti-50Al-15Cr coating after oxidation consisted of A12O3, whereas oxide formed on the surface of Ti-50Al-10Cr coating after oxidation is composed of a mixture of a large portion of A12O3 and a small portion of TiO2 that decrease the oxidation resistance. A review of advanced coatings on high temperature applications, including TiAl based and TiAl3 based alloys has been performed by [2006Nar]. Papers concerned with investigations of material properties are listed in Table 3.
Miscellaneous Interest in the Al-Cr-Ti system was focused on Ti rich alloys. When alloyed with Al and other transition metals, Ti rich alloys can exhibit martensitic transformation from α to β when quenched from the single-phase β-region [1953Bus]. Several studies were concentrated on the nature, kinetics and mechanism of this transformation [1953Bus, 1956Boe, 1956Zwi, 1963Wei]. The results were summarized in the form of T-T-T diagrams for β to α transformation. The growth kinetics of a discontinuous coarsening of lamellar structure in Ti-44Al-0.5Cr (at.%) intermetallic compounds was studied by [1998Jun]. The growth rate is linear during Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
7
8
7
Al–Cr–Ti
the initial period of the reaction and reaches a maximum near the eutectoid temperature. The migrating grain boundary plane maintains no definitive geometrical angular relationship to the lamellar interface. The discontinuous coarsening occurs through the grain boundary diffusion and its activation energy is estimated to be about 230 kJ·mol–1. This kinetic analysis suggests that the driving force for grain boundary migration is the elastic strain energy rather than the chemical and interfacial free energies, despite the comparatively larger value of the last two. Microstructural instability in a fully lamellar Ti-46.5Al-4Cr (at.%) during short-term creep was studied by [2000Cha] under creep tests at 175 MPa and 800˚C. Within Cr depleted regions α2 lamellae transform to γ by different mechanisms. In contrast, Cr enriched regions exhibit a transformation from the ordered hexagonal α2 to a cubic ordered B2 phase through a metastable Cr enriched α2 phase. [2001Lee] studied the general behavior of the CCTs for the Cr-containing alloy (Ti-45Al-2Cr (at.%)) at cooling rates from about 0,5 to about 500˚C·s–1 are similar; the α → γL lamellar reaction predominates at slow cooling rates, and only the α → α2 ordering reaction occurs at fast cooling rates; no massive transformation occurs at intermediate cooling rates. The addition of Cr to the Ti-45,5Al (at.%) binary alloy results in a simple displacement of the CCT curves of the α → γL lamellar reaction towards somewhat lower temperatures, in partial agreement with the depression of a transus temperature. Peculiarities of massive transformation in TiAl-based alloys were studied by [2001Xia]. [2000Wel] used mechanical spectroscopy and creep testing to measure activation enthalpies of viscoelastic relaxation in Ti-46.4Al-4Cr (at.%) alloy. They were determined as 3.9 and 3.6 eV, respectively, which are in the range of those obtained for self-diffusion. Thus, it can be assumed that grain boundary controlled diffusional creep is a dominating process at 800˚C and low stresses. The results indicate that the mechanical properties of Ti-46.5Al-4Cr (at.%) sheet material at 700–800˚C and high stresses are controlled volume diffusion assisted climb of dislocations. [2001Ish] studied opportunity to reduce the hydrogen desorption temperature of Ti3AlHx by substituting Ti with Cr. It was shown that the hydrogen capacity was largely reduced, but the hydrogen desorption temperature was unchanged or increased. Therefore Cr is the worst substitutional element to Ti3Al. The solidification-path of various Al-Cr-Ti alloys, which crystallized (Al,Cr)3Ti as the primary phase, were analyzed by [2001Mor, 2003Mor] using the data of Al-Cr-Ti phase diagram, k-values - functions of composition, and diffusion coefficient obtained by experiment. [1999Yan, 2000Yan] reviewed recent theoretical and experimental investigations of sublattice substitution of alloying element (Cr,V, Mn, Fe, Nb and others) in TiAl and Ti3Al phases. Electronic structure calculations for TiAl3-Cr alloys were performed by [1996Liu] and for TiAl-Cr alloys by [1996Woo] and obtained results were related to mechanical properties. [2007Hes] investigated pre-deformation microstructures, including lamellar, duplex and feathery structures, and microsctructures obtaining after hot forging of Ti-47Al-2Cr alloy. TEM investigations of TiAl based alloys were performed by [1994Zhe, 1994Gao, 1997Mas, 2005App].
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 1 Investigations of the Al-Cr-Ti Phase Relations, Structures and Thermodynamics Temperature/Composition/Phase Range Studied
Reference
Method / Experimental Technique
[1953Bus]
Homogenezation at 1000˚C, isothermal heat treatment, quenching, optical microscopy
Vertical section 550–1050˚C at constant Ti 5 mass% and Al in the range of 1–5 mass% Ti-3Al-5Cr (mass%), T-T-T diagram
[1953Tay]
XRD, metallography
980, 760˚C, 60–100% Ti isothermal sections
[1958Kor]
Arc-melting, heat treatment in vacuum, DTA, XRD, metallography, hardness, electrical resistivity
Liquidus isotherms 1400–1690˚C, isothermal sections at 600–1200˚C; 60–100% Ti
[1958Tag]
Phase equilibrium studies, metallography, XRD
600, 720, 850 and 1000˚C, 70–100 at.% Ti; isothermal sections and vertical section at Cr/Al=1, constant Cr 3.5 at.%, constant Ti 83 at.%
[1960Enc]
Phase equilibrium studies, metallography, XRD
600–1400˚C, 60–100 at.% Ti
[1960Zol]
X-ray analysis
Al alloy with 0.2% Ti and 2% Cr (mass%). The solubility of Ti in CrAl7
[1963Luz]
Homogenezation at 930˚C, annealing, electrical resistivity and hardness measurements
600–700 and 800˚C, solubiliy of Cr in Ti-6Al (mass%) alloy
[1964Ram]
XRD
As-cast and after annealing at 700˚C; AlCr2-AlTi2 (Ti: 7–50 at.%)
[1974Zwi]
Dilatometery
Annealing at 980˚C for 4 h and 760˚C for 10 d, Ti rich region, isothermal sections
[1978Jac]
X-ray
Ti(AlxCr1–x)2 at 0≤ x≤0.2, hydrogen sorption at 25˚C
[1984Sup]
XRD
Homogenezation at 1000˚C, heat treatment at 800˚C, TiCr2-TiAl2 solid solutions
[1988Gro]
Compacting and homogenizing in vacuum. Electron microprobe method, CALPHAD calculation
Annealing at 1100˚C for 4 h, then long period at 800˚C and quenching in water. Ti rich region, tie lines and calculated isothermal section.
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
9
10
7
Al–Cr–Ti
. Table 1 (continued) Temperature/Composition/Phase Range Studied
Reference
Method / Experimental Technique
[1990Zha]
Arc melting after cold isostatically pressed at 350 MPa powders and then hot isostatically pressed (HIPping) at 1200˚C and 175 MPa, 4 h in argon. Optical microscopy, SEM, energy dispersive spectrometry (EDS), X-ray diffraction, microhardness, DTA
[1991Mab]
XRD, TEM, SEM/EDX, DTA, microhardness Al-(20 to 80)Cr-50Ti (at.%). Isothermal section at 1000˚C
[1991Moh]
Arc-melting, homogenization at 1200˚C. 1300˚C, Ti-51Al-2.1Cr; site occupancy equilibration, quenching X-ray of Cr microanalysis, TEM
[1991Par]
Arc-melting, cyclic oxidation furnace at 1200˚C, gravimetry, XRD, SEM
1200˚C, Al67Cr8Ti25; oxidation resistance
[1991Spa]
Bulk ingots, arc melting, homogenization at 1200˚C for 16 h, X-ray diffraction, EPMA.
After homogenization. Ti27.6Cr6.8Al65.6 alloy.
[1992Dur]
Engel-Brewer theory
Al67Ti25Cr8 calculation of electron concentration
[1992Kim]
Arc-melting, annealing at 1050˚C in vacuum, forging at 1200˚C In situ XRD, optical microscopy, EPMA
1200˚C, Ti-48Al-2Cr (at.%)
[1992Mor]
HIP-treatment at 1140˚C and 100 MPa, spray deposition XRD, TEM
Al67Ti25Cr8 ordering
[1992Nic]
Bulk alloys, arc-melting from pure elements. HIPping at 1200˚C and 172 MPa, 2 h, in argon. X-ray diffraction, electron microprobe, EDS, hardness.
As-HIPed alloys. Al-Cr-50Ti (at.%). Isothermal section at 1200˚C.
[1992Win]
Bulk alloys, induction melting in argon, Ti25Cr8Al67. Crystal structure and lattice then homogenization at 1050˚C - 72 h in parameter of as-cast and homogenizated samples. vacuum. Optical microscopy, scanning electron microscopy, X-ray diffraction, EDS
[1992Zhe]
Bulk alloys, arc-melting, homogenization Annealing 1150–1200˚C for 24–168 1000˚C for 168 h in vacuum. Optical h in argon and cooling in air. microscopy, X-ray diffraction, SEM, TEM, Ti-44.3Al-3Cr (at.%). Phase composition. EDAX, microhardness.
[1993Ers]
Calculation, using the Linear Muffin Tin Orbital Method
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
As-HIPed alloys. Ti25Cr8Al67, Ti25Cr9Al66, stress-strain behavior
TiAl, Ti25Cr25Al50, Ti50Cr25Al25
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 1 (continued) Reference
Method / Experimental Technique
Temperature/Composition/Phase Range Studied
[1993Hao]
Diffusion couple technique, optical microscopy, EPMA.
[1993Nak]
1.Powder mixtures obtained at about As-homogenizated alloys. The range 260 MPa and sintered in vacuum at 1000 Al-(20 to 80)Cr-50Ti (at.%), isothermal or 1150˚C for 12 or 24 h. sections. 2.Bulk alloys, arc-melting, homogenization at 1150˚C for 2 days in vacuum. X-ray diffraction, optical microscopy, SEM, EDS.
[1994Boh]
Annealing in vacuum, XRD, SEM/EDX (backscattered)
700–1000˚C, Ti-48Al-2Cr (at.%)
[1994Kla]
Bulk alloys, arc melting from pure elements, HIPping at 1200˚C, 172 MPa, 2 h, X-ray diffraction, EPMA, backscattered electron imaging, EDS, hardness.
As-HIPed alloys. The range Al-(20 to 80) Cr-50Ti (at.%), isothermal section.
[1994Sok]
Arc melting from pure elements under Al-corner at up to 25 at.% Ti and 20 at.% Ar atmosphere. X-ray and microstruture Cr. Quenching in ice water after analyses annealing at 497˚C for 1000 h. Isothermal section.
[1994Zha]
Bulk alloys, arc-melting, homogenization As homogenizated alloy: Ti-42Al-3Cr at 1100˚C for 30 h and then 1050˚C for (at.%), phase composition 30 h. TEM, SEM, X-ray diffraction
[1994Zhe]
TEM
[1995Bra]
Bulk alloys, arc melting. X-ray diffraction, Heat treating at 1200˚C for 100 hours SEM, microhardness. in a 95%Ar-5%H2 and then furnace cooling. Heat treating in air at 800˚C for 100 hours and then air cooling to room temperature. Two alloys: Ti40Cr15Al45 and Ti30Cr15Al55. Phase composition.
[1995Hao]
Diffusion couples. EPMA, X-ray diffraction
The range Ti-(0 to 70)Cr-(0–75) Al (at.%). Isothermal section at 1000˚C.
[1995Jew]
Bulk alloys and diffusion couple technique. X-ray diffraction, optical microscopy, SEM, EDX.
Annealing at 800˚C for 750 h or 1000˚C for 650 h and then water quenching. Cr rich region: Cr-(0 to 70)Ti-(0–30)Al (at.%). Isothermal sections, phase equilibria at 800 or 1000˚C.
[1995Kog]
Arc-melting, homogenization at 1100˚C, 1100˚C; 17 alloys Al-(25–28)Ti-(9–14)Cr annealing, quenching, XRD (at.%)
Landolt‐Bo¨rnstein New Series IV/11E1
Annealing 1000˚C for 200 h, 1000˚C 100 h in vacuum. The range Ti-(20–80)Cr-50Al (at.%). Isothermal section
25˚C, Ti-45Al-3Cr (at.%)
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
11
12
7
Al–Cr–Ti
. Table 1 (continued) Reference
Method / Experimental Technique
Temperature/Composition/Phase Range Studied
[1995Nak]
Arc-melting, XRD, optical metallography, 1200˚C, Ti-48Al-2(Cr, Mo, Mn) (at.%) SEM, TEM, EPMA
[1996Jew1]
Thirteen bulk alloys, arc-melting, homogenization in vacuum for 2 h at 1380˚C or 1270˚C and furnace cooling. Optical microscopy, SEM, EDX, X-ray diffraction, DSC for enthalpy determination.
Annealing at 800˚C for 1000 h or 1000˚C for 500 h, then water quenching. Cr-Ti rich alloys with 0 to 30 at.% Al. Isothermal section, phase equilibria at 800 and 1000˚C, tie lines.
[1996Jew2]
Eleven bulk alloys, arc-melting, homogenization in evacuated ampules at 1140 or 1250˚C for 3 to 4 h. Diffusion couple technique. Optical microscopy, SEM, EDX, X-ray diffraction, DSC measurements.
Annealing 800˚C for 100 to 1000 or or 1000˚C for 100 to 500 h, respectively, and water quenching. Al-(0 to 80)Cr-40Ti (at.%) alloys. Isothermal section, phase equilibria at 800 and 1000˚C.
[1997Mab1], [1997Mab2]
Compact samples from powders, sintering in vacuum for 48 h at 1200˚C, then blowing-air quenching. Button ingots, arc-melting, homogenization at 1200˚C in vacuum for 2 d, then aircooling. X-ray diffraction, optical microscopy, SEM, EDX, DTA, microhardness, bend testing.
After homogenization (isothermal section) or heat treatment: 1300˚C for 2 h, 1250˚C for 4 h, 1150˚C for 48 h, 1000˚C for 144 h, then water quenching (vertical section). Al-(0 to 70)Cr-(0 to50)Ti (at.%). Isothermal section at 1150˚C and vertical section for Al-25Ti-(0–28)Cr (at.%).
[1997Fan]
Mechanical alloying for 40 h of milling. X- Heat treating at 700˚C and cooling to ray diffraction, TEM, DSC. room temperature. The Al-25Ti-8Cr (at.%) alloy.
[1997Jew]
Twelve bulk alloys, arc-melting, homogenization in vacuum at temperature below solidus for 2 to 4 h, then furnace cooling. Optical microscopy, SEM, EDX, X-ray diffraction, DSC measurements.
Annealing 800˚C for 100, 150 and 1000 h or 1000˚C for 100,160 and 500 h, then water quenching. Isothermal section at 800 and 1000˚C, temperature of invariant reaction.
[1997Par]
Six button ingots, arc melting, homogenization at 1150˚C for 48 h in vacuum, then furnace cooling. X-ray diffraction, EDX, optical microscopy, SEM, compression tests.
After homogenization. Al-(21 to 30)Ti-(6, 15, 23)Cr (at.%). Isothermal section at 1150˚C.
[1997Xu]
Diffusion couple TiAl3-Cr and diffusion triples Cr-Ti-TiAl3. Optical microscopy, SEM, EDX.
Annealing at 1050˚C for 496 or 532 h. Isothermal section at 1050˚C.
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 1 (continued) Temperature/Composition/Phase Range Studied
Reference
Method / Experimental Technique
[1998Has]
Bulk samples, arc melting. Diffusion couple technique. Homogenization at 1050˚C (bulk) and 1100˚C (diffusion couple) for 345.6 ks in vacuum, then furnace cooling. Optical microscopy, X-ray diffraction, EPMA, DTA. Calculation with Thermocalc program.
Heat treatment at 1200˚C for 172.8 ks, then ice water quenching. Ti rich region. Calculation of isothermal section at 1200˚C and phase equilibria between αTi, β and TiAl phases at 1200˚C accoding to experimental data.
[1998Jun]
Button ingots, arc melting, homogenization at 1330˚C for 3 h and air cooling. Optical microscopy, X-ray diffraction, TEM.
Aging treatment at 650 to 1200˚C. The Al-44Al (at.%) alloy with 0.5 at.% Cr. Lattice parameters of Ti3Al and TiAl phases at various temperatures.
[1999Hao]
Arc-melting, homogenization at 900˚C, quenching, electron microscopy/EDAX
900˚C, Ti-(46–53)Al-(1–5)Cr (at.%)
[1999Jac]
Vapour-pressure measurements (Knudsen cell)
1000–1400˚C, Ti-47Al-2Cr, Ti-47Al-13Cr, Ti-51Al-12Cr
[1999Nic]
Arc-melting, HIP at 1200˚C and 172 MPa, 1200˚C, Al-25Ti-(9,12)Cr, EPMA, XRD Al-(23,27)Ti-10Cr (at.%)
[1999Sha]
Bulk ingot, arc melting. Melt-spun ribbon. EPMA, TEM, EDXA, calculation phase equilibria.
[2000Kai1]
Bulk ingot, arc melting, homogenization Annealing at 1000˚C for 168 h and ice 1200˚C for 3 h. Diffusion couple. SEM, water quenching. Ti-(15 and 18 to EDS, TEM, optical microscopy. 27)Al-(3 and 5)Cr (at.%). Phase equilibria at 1000˚C in the (βTi) region.
[2000Cha]
Powder metallurgical process, heat treatment in vacuum, creep-testing, TEM,TEM/EDX, SEM
800˚C, Ti-46.5Al-4(Cr,Nb, Ta, B) Influence of creep to microsctructure instability
[2000Kai2]
Bulk ingot, arc melting. EPMA.
Annealing at 1000˚C for 168 or 504 h, at 1200˚C for 168 h, at 1300˚C for 24 h, then ice water quenching. Ti rich region: Ti-(35 to 47)Al-(0.5 to12)Cr (at.%). Phase equilibria at 1300, 1200, 1000˚C between (αTi), β, TiAl.
[2000Sha]
Bulk ingots, arc melting, melt-spun ribbons. EPMA, TEM, EDX.
After casting and after annealing at 450˚C for 100 h. Ti-(20 to 52)Al-(7.5 to 20)Cr (at.%). Metastable β-based structures.
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
Ti-40Al-10Cr (at.%), Ti-50Al-10Cr (at.%), Ti-52Al-20Cr (at.%). Phase equilibria at 1000˚C, calculated liquidus surface projection and isothermal section at 1000˚C.
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
13
14
7
Al–Cr–Ti
. Table 1 (continued) Reference
Method / Experimental Technique
Temperature/Composition/Phase Range Studied
[2001Fuj]
X-ray diffraction, TEM, optical microscopy
Heat treatment at 1200˚C for 4 d, 1000˚C for 7 d, the ice water quenching. 13 alloys in Ti rich region with (38 to 60) at.% Al, (0 to 21) at.% Cr. Phase equilibria at 1200 and 1000˚C.
[2001Ich]
DTA, XRD, isothermal heat treatment
1250–1350˚C, 50–100 at.% Al (liquidus and solidus τ1 and vertical section at Ti 25 at.%)
[2001Kan]
Calculation of phase equilibrium by cluster variation method.
Calculation TiAl/Ti3Al and αTi/Ti3Al phase boundaries at 1000˚C in Al-Cr-Ti phase diagram.
[2001Kau]
CALPHAD method
Isothermal sections at 1500, 1300, 1200, 1000˚C, phase fraction diagram for Al15Cr4Ti7 and vertical section from Al to Ti-50 at.% Cr
[2001Lee]
Arc-melting, homogenezation at 1200˚C 900–1200˚C, Ti45Al-2Cr, kinetic study in vacuum, TEM
[2001Sun]
Bulk ingots, arc melting, HIPping at Annealing 900˚C for 8 h and air cooling. 1200˚C for 3 h, heat treatment at 1200˚C Ti52Al48–xCr (x = 0, 1, 2, 4, 6). Phase equilibria between Ti3Al, TiAl, τ3. for 12 h, air cooling. X-ray diffraction, XPS, TEM, SEM, EPMA, tensile test, creep test.
[2001Yam], [1999Yam]
Arc-melting, homogenezation at 1177˚C 1177˚C, in vacuum, quenching; XRD, optical Al-(9.24–12.32)Cr-(25.38–26.71)Ti (at.%) microscopy, SEM, EPMA
[2003Bar]
Bulk ingots, arc melting. Optical As-cast alloys. Al-(14 to 27) at.%Ti-(11 to microscopy, SEM, X-ray diffraction, DTA, 35) at.%Cr. Univariant equilibria with hardness, compression test, Young’s liquid phase. modulus.
[2003Lee]
Arc-melting, homogenization at 1150˚C 800˚C; Al-21Ti-23Cr, Al-21Ti-15Cr, in vacuum 10–1 Pa, XRD, TEM, SEM/EDX, Al-30Ti-15Cr optical microscopy
[2003Mor]
Progressive type of solidification equation based on experimental data on phase diagram, partitioning coefficients, diffusion coefficients
[2003Nis1], [2003Nis2]
Bulk ingot, arc melting. EPMA, SEM, X-ray Coated by Cr at 1300˚C and Al at diffraction, oxidation resistance studies 1000–1300˚C and air quenching. Melted and hardness measurements. samples were annealing at 1000˚C for 86.4 ks. Phase equilibria between τ1, τ2, β, TiAl.
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Calculation of solidification path (1250–1350˚C) of various Al-Cr-Ti alloys with Ti content of 15–29 at.% and Cr content of 6–20 at.%
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 1 (continued) Reference
Method / Experimental Technique
Temperature/Composition/Phase Range Studied
[2003Ram]
Cr and Ti magneton sputtering on Al 600, 700˚C heat treatment, target - thin films EPMA, SEM, XRD, TEM, TiAl-(0.6–4.6)Cr gravimetry
[2004Nay]
Mechanical alloying for 40 h of milling. X- After milling. The Cr8Ti27Al67 alloy. Lattice parameters. ray diffraction, TEM.
[2004Wan]
Skul melting, XRD, SEM/BSE, EPMA
Ti-46Al-8Cr-2.65(Nb,W,B)
[2007Hes]
Arc-melting, vacuum heat treatment, cooling in air, TEM, SEM and optical microscopy
1100˚C homogenization, 1400˚C heat treatment, Ti-47Al-2Cr (at.%)
. Table 2 Crystallographic Data of Solid Phase Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
(Al) < 660.452
cF4 Fm3m Cu
β, (βTi,Cr) < 1863
cI2 Im3m W
Lattice Parameters [pm]
dissolves up to 0.8 at.% Ti at 665.7˚C [2008Cor] and 0.35 at.% Cr at 661.5˚C [2007Wit] at 25˚C [Mas2]
a = 404.96
0 to 100 at.% Cr at 1410 to 1359˚C [2008Iva] dissolves up to 40 at.% Al at 1000˚C [1999Sha] for Ti6.5Cr68.6Al24.9, quenched from 800˚C [1997Jew] for Ti12.9Cr58.0Al29.1, quenched from 800˚C [1997Jew] dissolves up to 46 at.% Al at 1350˚C [2008Cor] at 25˚C [Mas2] dissolves up to 49.4 at.% Al at 1491˚C [2007Wit] [V-C2]
a = 294.4 a = 294.6 (Cr) < 1863
a = 288.48
(βTi) 1670 - 882 a = 330.65 (αTi) < 882
Landolt‐Bo¨rnstein New Series IV/11E1
hP2 P63/mmc Mg
Comments/References
dissolves up to 51.4 at.% Al at 1456˚C [2007Wit] and 0.6 at.% Cr [2008Iva] a = 295.06 c = 468.35
at 25˚C [V-C2]
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
15
16
7
Al–Cr–Ti
. Table 2 (continued) Pearson Symbol/ Space Group/ Prototype
Phase/ Temperature Range [˚C] CrAl7 < 790
mC104 C2/m V7Al45
Cr2Al11 940 - 785
orthorhombic
oC584 Cmcm
Lattice Parameters [pm]
a = 2519.6 b = 757.4 c = 1094.9 β = 128.7˚C
Comments/References Cr2Al13 at room temperature 13.5 at.% Cr [2008Cor]
CrAl5 16.9 to 19.2 at.% Cr quenched from 920˚C [2008Cor]
a = 1240 b = 3406 c = 2020 a = 1252.1 b = 3470.5 c = 2022.3 a = 1260 b = 3460 c = 2000
single crystal “εCrAl4” [2008Cor]
CrAl4 < 1030
hP574 P63/mmc MnAl4
a = 1998 c = 2467 a = 2010 c = 2480
at room temperature, 20.9±0.3 at.% Cr [2008Cor] at Cr rich border at 1000˚C [2008Cor]
γCr4Al9 1170 - ≈1060
-
-
30 to 34 at.% Cr [2008Cor]
βCr4Al9 ≲ 1060
cI5 I43m Cu4Al9
a = 912.3
30 to 35 at.% Cr at Al rich border at 920˚C [2008Cor]
αCr4Al9 ≲700
hR156 R3m Cr4Al9
a = 1291 c = 1567.7
32.8 to 35 at.% Cr [2008Cor]
βCr5Al8 cI52 ≈1350 - ≈1100 I43m Cu5Zn8
35 to 42 at.% Cr, a = 910.4 to 904.7 quenched from liquid [2008Cor]
αCr5Al8 ≲ 1160
hR78 R3m Cr5Al8
a = 1281.3 c = 795.1
Cr2Al < 910
tI6 I4/mmm MoSi2
≈ 65.5 to ≈ 71.4 at.% Cr a = 300.5 to 302.8 [2008Cor] c = 864.9 to 875.5
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
35 to 42 at.% Cr [2008Cor]
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 2 (continued) Pearson Symbol/ Space Group/ Prototype
Phase/ Temperature Range [˚C]
Lattice Parameters [pm]
Comments/References
X ≲ 400
Cr5Al3 or Cr3Al super lattice
-
≈ 75 to ≈ 80 at.% Cr possibly metastable [2008Cor]
w
-
-
In quenched alloy of 60 to 100 at.% Cr, like metastable wTi [2008Cor]
γTiCr2 1359 - 1269
hP12 P63/mmc MgZn2
a = 493.2 c = 800.50
Laves phase C14 at 25˚C for Ti1.12Cr2 [2008Iva]
βTiCr2 1271 - 804
hP24 P63/mmc MgNi2
αTiCr2 < 1223
cF24 Fd3m MgCu2
ωTi Cr2 < 450
hP3 P3m1 ωTiCr2
β0 1427–1159
cP2 Pm3m CsCl
Laves phase C36. Dissolves up to 4 at.% Al [1996Jew1] at 25˚C [2008Iva]
a = 493.2 c = 1601.0
Laves phase C15. Dissolves up to 1 at.% Al [1997Xu] at 25˚C for TiCr1.9 [2008Iva]
a = 693.20
from 3 to 9 at.% Cr, metastable phase [2008Iva] at 4.6 at.% Cr
a = 461.6 c = 282.7
high temperature ordered B2 phase [2007Wit]
-
hP8 α2, Ti3Al < 1293 P63/mmc (up to 10 GPa) Ni3Sn
from 18 at.% Al at 600˚C to 38.5 at.% Al at 1119˚C D019 ordered phase (α2-Ti3Al) [2007Wit] dissolves up to 2.5 at.% Cr at 800 to 1000˚C [1997Jew] at 25 at.% Al [2006Sch]
a = 576.5 c = 462.5
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
17
18
7
Al–Cr–Ti
. Table 2 (continued) Phase/ Temperature Range [˚C] γ, TiAl < 1456
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
tP4 P4/mmm AuCu
from 46.7 at.% Al at 1119˚C to 62.1 at.% Al at 1432 at.% Al [2007Wit] L10 ordered phase (γ-TiAl) Dissolves up to 8 at.% Cr at 1000˚C and up to 4.5 at.% Cr at 800˚C [1997Jew] at 50.0 at.% Al [2006Sch]
a = 400.0 c = 407.5 a = 400.6 c = 406.1 a = 398.1 c = 406.6 a = 400.5 c = 406.3 a = 399.0 c = 406.1 η, TiAl2 < 1224
ζ, Ti2Al5 1432 - 976
tI24 I41/amd HfGa2
tetragonal super structure of AuCu-type
ε (h), TiAl3(h) 1396 - 734
tI8 I4/mmm TiAl3(h)
ε (l), TiAl3(l) < 932
tI32 I4/mmm TiAl3(l)
TiAl3(m)
cP4 Pm3m AuCu3
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
Comments/References
for Ti51.0Cr1.7Al47.3, quenched from 1000˚C [1997Jew] for Ti36.6Cr8.0Al55.4, quenched from 1000˚C [1997Jew] for Ti50.9Cr2.0Al47.1, quenched from 800˚C [1997Jew] for Ti48.2Cr4.2Al47.6, quenched from 800˚C [1997Jew] dissolves about 2.3 at.% Cr at 976˚C [2007Wit] for TiAl2 [2006Sch]
a = 397.0 c = 2497.0 a = 396.1 c = 2415.2 a = 395.2 c = 2411.7
for Ti34.3Cr3.5Al62.2, quenched from 1000˚C [1997Jew] for Ti34.2Cr3.1Al62.7, quenched from 800˚C [1997Jew] from 65 at.% Al at 1432˚C to 70.4 at.% Al at 1396˚C [2007Wit]
a = 392.30 c = 1653.48 a = 390.53 c = 2919.21
at 68.75 at.% Al [2006Sch] at 71.4 at.% Al [2006Sch] from 74.2 at.% Al at 1396˚C to 76.5 at.% Al at 734˚C [2007Wit] [2006Sch]
a = 384.9 c = 861
from 74.6 at.% Al at 932˚C to 75.7 at.% Al at 665.7˚C [2007Wit] [2006Sch]
a = 387.7 c = 3383.2 a = 397.2 a = 396.7
by splat cooling [2006Sch] by mechanical alloying [2006Sch]
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 2 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Ti3Al5 < 810
tP32 P4/mbm Ti3Al5
* τ1, (Ti1–x+yCrx) Al3–y ≲ 1370
cP4 Pm3m AuCu3
Lattice Parameters [pm] a = 1129.3 c = 403.8
[2006Sch]
L12 ordered phase stabilized by Cr at 7 to 13 at.% Cr at 1200˚C [1992Nic], at 0.28 ≤ x≤ 0.48 and 0≤y≤0.68 at x = 0.32, y = 0.32 for Ti25Cr8Al67, annealed at 1200˚C [1992Nic] at x = 0.32, y = 0,32 for Ti25Cr8Al67, as-cast [1990Zha] at x = 0.272, y = 0.376 for Ti27.6Cr6.8Al65.6, annealed at 1200˚C [1991Spa] at x = 0.32, y = 0.32 for Ti25Cr8Al67 annealed 800˚C [1992Win] at x = 0.32, y = 0.32 for Ti25Cr8Al67, mechanical alloying for 40 h, annealed 700˚C [1997Fan] at x = 0.32, y = 0.32 for Ti25Cr8Al67 mechanical alloying for 40 h [2004Nay] at x = 0.476, y = 0.588 for Ti27.8Cr11.9Al60.3, quenched from 1000˚C [1997Jew] at x = 0.42, y = 0.656 for Ti30.9Cr10.5Al58.6, quenched from 1000˚C [1997Jew]
a = 395.4
a = 395.4 a = 395.8
a = 396.3
a = 396.3**
a = 397.3**
a = 394.5
a = 395.1
Landolt‐Bo¨rnstein New Series IV/11E1
Comments/References
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
19
20
7
Al–Cr–Ti
. Table 2 (continued) Phase/ Temperature Range [˚C] * τ2, Ti(Cr,Al)2 < 1200
* τ3 < 1050
Pearson Symbol/ Space Group/ Prototype hP12 P63/mmc MgZn2
cP2 Pm3m CsCl
Lattice Parameters [pm]
Comments/References C14 ordered phase stabilized by Al
a = 495** c = 805** a = 503** c = 820.7** a = 504.42 c = 824.62 a = 505.5 c = 827.8 a = 504.7 c = 825.3 a = 504.3 c = 824.3 a = 504.5 c = 824.1 a = 502.8 c = 821.3 a = 492.6 c = 803.2 a = 493.2 c = 803.6 a = 495.6 c = 809.0
for Ti33..3Cr56.7Al10 at 1000˚C [1996Jew1] for Ti33..3Cr36.7Al30 at 1000˚C [1996Jew1] for Ti31.5Cr26.7Al41.8, quenched from 1000˚C [1997Jew] for Ti33.6Cr29.3Al37.1, quenched from 1000˚C [1997Jew] for Ti35.8Cr30.2Al34.0, quenched from 1000˚C [1997Jew] for Ti31.6Cr29.3Al39.1, quenched from 800˚C [1997Jew] for Ti33.3Cr27.6Al39.0, quenched from 800˚C [1997Jew] for Ti34.2Cr34.5Al31.3, quenched from 800˚C [1997Jew] for Ti33..3Cr61.2Al5..5 as-cast [1978Jac] for Ti33..3Cr56.7Al10 as-cast [1978Jac] for Ti33..3Cr53.4Al13..3 as-cast [1978Jac] B2 ordered phase stabilized by Cr for Ti56.9Cr7.6Al35.5, quenched from 1000˚C [1997Jew] for Ti52.2Cr13.3Al34.5, quenched from 1000˚C [1997Jew] for Ti46.5Cr21.6Al31.9, quenched from 1000˚C [1997Jew] for Ti53.9Cr14.1Al53.9, quenched from 800˚C [1997Jew] for Ti46.9Cr20.8Al32.3, quenched from 800˚C [1997Jew] for Ti55Cr3Al42, annealed at 1050˚C [1994Zha] for Ti50Cr25Al25 [1964Sch]
a = 316.3 a = 315.0 a = 312.8 a = 315.4 a = 313.3 a = 319.7 a = 312
Note: ** - Lattice parameters are derived from figures
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 3 Investigations of the Al-Cr-Ti Materials Properties Reference
Method / Experimental Technique
Type of Property
[1963Luz]
Resistivity measurements, hardness
Solubility of Cr in Ti-6 mass% Al, electrical and mechanical properties
[1978Jac]
Sivert’s method
Hydrogen capacity of Ti(Cr1–xAlx) (0≤x≤0.2) at 7 MPa, 293 K and 4 MPa, 80 K
[1984Sup]
Faradey microbalance method
The temperature dependence of magnetic susceptibility of TiCr2 - TiAl2 alloys
[1990Mab]
Hot-pressed compact specimens, TEM, X- Compression tests at temperatures from ray diffraction, Vickers microhardness, 300 to 1300 K of Ti25Cr8Al67 with L12 structure compression tests at elevated temperature
[1990Zha]
Light microscopy, SEM, DTA, compressing tests, Vickers hardness
[1991Bea]
Arc-melting, HIP at 1220˚C, hot-rolling at 1300˚C, Ti48Al-2Cr 1260˚C or forging at 1025, heat treatment, optical microscopy, SEM
[1991Hua]
Light microscopy, AEM, 4-point bending Effect of alloying with Cr on the and tensile test microstructure and plasticity of Ti-(45–54) Al-(1–4)Cr (at.%) alloys prepared as meltspun ribbon, consolidated by cold compaction, HIPped and extruded
[1991Mab]
X-ray diffractometry, TEM, SEM, mechanical testing
[1991Mae]
Mechanical properties of Ti-35.5Al-1.5Cr Tensile tests at room temperature and 1073 K with a strain rate of 8.3·10–5·s–1. (at.%) at room temperature and 800˚C Creep rupture tests were carried out on the as cast materials at 800˚C in air with the applied stress between 180–250 MPa.
[1991Mas]
Temperature and strain rate Mechanical properties of γ (TiAl)-based dependencies of the tensile properties alloy cointaining bcc phase of were examined by tensile tests in Instron composition of Ti-47Al-3Cr (at.%) type machine. Compression tests for isothermally forged alloys were carried out below 1073 K at 7.5·10–4 sec–1 initial strain rate. The deformed and fractured specimens were characterized by optical microscopy, SEM, TEM and XRD (diffraction and photograph).
Landolt‐Bo¨rnstein New Series IV/11E1
Mechanical properties of as-casted and HIPped alloys of Ti25Cr8Al67 and Ti25Cr9Al66
Mechanical properties of Ti25Cr8Al67 at 400–1000˚C
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
21
22
7
Al–Cr–Ti
. Table 3 (continued) Reference
Method / Experimental Technique
[1991Mik]
Hardness (HDP), compression and bend testing, ultrasonic vawe velocity measuremenrs, dilatometry
Mechanical properties, including elastic moduli; average coefficient of thermal expansion for temperature interval 200–1200˚C foras cast and HIPped Ti25Cr8Al67
[1991Nic]
Hardness (HDP), compression and bend testing, ultrasonic wave velocity measuremenrs
Hardness, crack loading, Young’s modulus of Ti25Cr8Al67
[1991Par]
Tests in cyclic oxidation furnace in static air at 1200˚C for 200 cycles: 1 h immersion at 1200˚C followed by 20 min cool down to rome temperature
Oxidation resistance of Ti25Cr8Al67 at 1200˚C
[1992Miz]
Tensile tests at 1200˚C at an initial strain Annealing time dependence of tensile strength and elongation in isothermally rate 5.4 · 10–4 s–1 forged Ti-46.1Al-3.1Cr (at.%) at 1200˚C. Annealing time from 0 to 170 h
[1992Mor]
Hardness, toughness testing in a range of Mechanical properties loads
[1992Nic]
Hardness (DPH)
Hardness profile and load necessary to couse cracks for 25Ti-Al-xCr 0<x<20 at.% in as cast and HIPped states
[1992Zhe]
Microhardness
Microhardness of phases in Ti-44.3Al-3Cr (at.%) alloy
[1993Has]
Tensile test, strain rate 10–4·s–1
Yield stress, fracture stress, elongation and Yong’s modulus at ambient temperature of Ti-48.7Al-1.3Cr (at.%) alloy annealed at 1350˚C for 1 h
[1993Kaw]
Four-point bend tests at room temperature at strain rate 10–3·s–1
The effect of Ti/Al ratio and Cr additions on mechanical properties in TiAl-base alloys
[1993Nak]
Vickers microhardness using a 25 g load, three-point bend tests at ambient temperature using an Instron mashine at a constant cross-head deflection rate of 0.1 mm·min–1
Mechanical properties of sintered specimens of Ti25Cr8Al67, Ti25Cr9Al66 and melted button ingots of Ti25CrxAl75–x, where x=8, 13, 14 and 16 at.% as a function of phase composition, and porosity
[1993Wri]
Hardness (HDP)
Hardness as a function of aging temperature for 1 h heat treatments of Ti27.5Cr8Al27.5 after solution treatment for 1 h at l000˚C and oil quenched
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Type of Property
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 3 (continued) Reference
Method / Experimental Technique
Type of Property
[1994Kla]
Hardness (HDP)
Constructing of contour map of hardness values and contour map of cracking resistance load for Al-Ti50Al50Ti50Cr30Al20-Cr80Al20 composition region
[1994Li]
Conventional tensile tests were carried out at room temperature in air using a servohydraulic Instron model 8500 testing machine equipped with a digital control unit
Tensile properties of as HIPped Ti-44Al-2Cr alloy
[1995Bra]
Heat treating in air at 800 and 1000˚C for High temperature oxidation resistance of 100 h Ti-45Al-15 Cr and Ti-55Al-15Cr (at.%) alloys
[1995Whi]
Compression, creep test
Mechanical properties at elevated temperatures for alloys Al-25Ti-9(Cr, Fe, Mn)
[1996Jew1] Hardness (HDP)
Variation of hardness of the Ti(Cr,Al)2 phase with composition
[1997Hei]
The hardness at temperatures up to 500˚C of oxide dispersion strengthened (3 vol.% Y2O3) Ti25Cr8Al67 produced by mechanical alloying and hot compressing at 800˚C
The elevated temperature Vickers hardness using 200 N load
[1997Mab2] Microhardness, bend test
Interrelations, between starting phase composition, porosity and ductility of TiAl3 alloyed with Cr
[1997Ley]
Interrupted weight gain tests in laboratory air at 750 and 900˚C
Oxidation behavior of Ti-Al-Cr coatings deposited by magnetron sputtering of Ti-(44 -66)Al-(4 -22)Cr (at.%) alloys
[1998Jim]
Strain-rate-change tests at strain rates ranging from 10 –6 to 10–3 s–1 in a universal testing machine. The mechanical tests were performed in compression in the temperature range from 800 to 1100˚C.
Mechanical properties at elevated temperatures of Ti-47Al-3Cr (at.%) alloy
[2000Cha]
Creep-test
Mechanical properties of Ti-46.5Al-4(Cr, Nb,Ta,B)
[2000Coe]
Hardness tests were carried out with loads of 70 and 300 mN in an ultramicroindentation device with a Vickers indenter
Mecanical properties of thing films TiAl-(0.6–4.6)Cr (at.%) produced by magnetron sputtering
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
23
24
7
Al–Cr–Ti
. Table 3 (continued) Reference
Method / Experimental Technique
Type of Property
[2000Mab]
Vickers hardness, bend tests, compressive tests
Mechanical properties of button ingots of Al-25Ti-5Cr-4V and Al-xTi-yCr-3V(x = 25, 27, 29, y = 6, 8, 10, 12, 14) alloys prepared by arc-melting
[2000Ohi]
Vickers hardness
Hardness and microstructural variations during aging of Al-Cr-Ti ternary Ll0- and Ll2-phase alloys
[2000Wel]
Subresonance torsion apparatus
Mechanical properties of Ti-46.5Al-4(Cr, Nb,Ta,B) consisting of TiAl and Ti3Al up to 1000˚C
[2001Ish]
Sorbtion and desorption of hydrogen
The effect of sustituting of Ti for Cr on the hydrogen capacity and desorption temperature of Ti75–xCrxAl25 (x = 0, 15, 25)
[2001Mil]
Young’s modulus, Vickers hot hardness, The Vickers hot hardness at load p = stress-strain curves of TiAl3 and 2.34 N, four-point bending tests at a Ti28Cr12Al61 cross-head speed of 0.2 mm· min–1, compression tests with a strain rate of 10–3·s–1, indentation method, using nine trihedral diamond indenters with tip angles of 45, 50, 55, 60, 65, 70, 75, 80 and 85˚C.
[2001Sun]
Tensile tests at room temperature and at 900˚C in air using an MTS testing machine, a nominal engineering strain rate of 2·10–3·s–1 was used for the tensile tests; creep tests were carried out at 800˚C
[2001Zho]
Isothermal oxidation tests at 900, 950 and Effect of Ti-50Al-15Cr and Ti-50Al-10Cr 1000˚C in static air. A thermal balance (at.%) coatings on the oxidation behavior was used to measure the weight change of TiAl alloys continuously. Cyclic oxidation tests using a cyclic oxidation furnace in static air at 950 and 1000˚C. Each cycle consisted of an hour immersion in static air in the furnace followed by a 20 min cool down to room temperature.
[2002Bra]
Vickers hardness was found with a Leco Effect of alloying with Cr on the M-400 hardness tester (1 kg, 20 s), three- mechanical properties of TiAl3, point-bend testing was adapted from the (Ti31Cr3Al66, Ti28Cr6Al66, Ti25Cr9Al66) ASTM standard C1161–94
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Effect of alloying with Cr on the microstructure, tensile properties and creep resistance of Ti52Al48–xCr alloys (x = 0, 0.5, 1.0, 2.0, 4.0, and 6.0 at.%
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Table 3 (continued) Reference
Method / Experimental Technique
Type of Property
[2002Cal]
Compression tests were made as a function of temperature in a vacuum atmosphere (<10–3 Pa). Most compression tests were carried out at a constant crosshead rate of 0.002 mm·s–1 and others at 0.0033 mm·s–1.
Evaluation of the mechanical properties of Ti50Al50, Ti50Al48Cr2, Al67Ti25Cr8 at temperatures ranging from 298 to 773 K. Nanocrystalline alloys have been produced by means of mechanical milling and spark plasma sintering.
[2003Bar]
The Vickers hardness at load 98 N; Young’s modulus was determined in four point bending tests at a cross-head speed of 0.2 mm/min, compression tests with a strain rate of 10–3·s–1
The analysis of mechanical properties under transition from single-phase L12 aloys to eutectic microstructures L12+β (Cr)
[2003Lee]
Compressive tests at room temperature using an Instron testing machine (Model 4206) at a strain rate of 1·10–1·s–1.Fracture toughness was obtained through threepoint bend test using an Instron testing machine (Model 4206) at a strain rate of 1·10–4·s–1 for single edges notched bend specimens.
Examination of the relationship between mechanical properties and phase stability of Al-21Ti-23Cr, Al-21Ti-15Cr and Al-30Ti-15Cr alloys proposed as coating materials with high oxidation resistanse
[2003Nis1] [2003Nis2]
Oxidation tests were carried out in air under a thermal cycling condition between 900˚C and room temperature.
Protective properties of three layer coatings for TiAl-based alloys
[2003Ram]
Microidentation
Microhardness of heat treated TiAl-based thing films alloyed with Cr up to 3 at.%
[2004Wan]
Strain-rate testing
Mechanical properties Ti-46Al-8Cr-2.65 (Nb,W,B) at 800–1100˚C
[2006Fox]
The isothermal interrupted oxidation tests in air, over a wide range of temperatures from 750 to 1100˚C
Oxidation resistance of TiAl3-based alloys alloyed with Cr
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
25
7
Al–Cr–Ti
. Fig. 1a Al-Cr-Ti. Partial reaction scheme, part 1
26
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
7
. Fig. 1b Al-Cr-Ti. Partial reaction scheme, part 2
Al–Cr–Ti
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
27
7
Al–Cr–Ti
. Fig. 1c Al-Cr-Ti. Partial reaction scheme, part 3
28
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
7
. Fig. 1d Al-Cr-Ti. Partial reaction scheme, part 4
Al–Cr–Ti
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
29
30
7
Al–Cr–Ti
. Fig. 2a Al-Cr-Ti. Tentative liquidus surface projection (solid lines - calculations, dashed lines experiments)
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Fig. 2b Al-Cr-Ti. Tentative liquidus surface projection, enlarged view of the Al corner
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
31
32
7
Al–Cr–Ti
. Fig. 3 Al-Cr-Ti. Partial isothermal section at 1300˚C
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Fig. 4 Al-Cr-Ti. Partial isothermal section at 1200˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
33
34
7
Al–Cr–Ti
. Fig. 5 Al-Cr-Ti. Tentative isothermal section at 1050˚C
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Fig. 6 Al-Cr-Ti. Isothermal section at 1000˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
35
36
7
Al–Cr–Ti
. Fig. 7 Al-Cr-Ti. Isothermal section at 800˚C
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Fig. 8 Al-Cr-Ti. Partial isothermal section at 600˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
37
38
7
Al–Cr–Ti
. Fig. 9 Al-Cr-Ti. Activities of Al in Ti-47Al-2Cr, Ti-47Al-13Cr and Ti-51Al-12Cr alloys according to the experimental data of [1999Jac]
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti
7
. Fig. 10 Al-Cr-Ti. Activities of Ti in Ti-47Al-2Cr, Ti-47Al-13Cr and Ti-51Al-12Cr alloys according to the experimental data of [1999Jac]
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
39
40
7
Al–Cr–Ti
References [1953Bus] [1953Han]
[1953Tay] [1956Boe] [1956Zwi]
[1958Tag] [1958Kor]
[1960Enc] [1960Zol]
[1963Luz]
[1963Wei] [1964Ram] [1964Sch] [1974Zwi] [1978Jac]
[1984Sup]
[1988Gro]
[1989Kim] [1990Lam]
[1990Mab] [1990Zha]
Busch, L.S., “Transformation Characteristics of 3% Al - 5% Cr Titanium Alloy”, J. Metals, 5, 146–149 (1953) (Morphology, Experimental, Phase Diagram, Phase Relations, Mechan. Prop., 2) Hansen, M., McPherson, D.J., Rostoker, W., “Constitution of Ti Alloy Systems”, ADC Techn. Rep. 53–41, Armour Res. Found. Illinois Inst. Techn., WADC TR 53–41, 129–136 (1953) (Phase Diagram, Phase Relations, 3) Taylor, J.L., Duwez, P., “Constitution of Titanium Rich Ti-Cr-Al Alloys”, J. Metals, 5, 253–256 (1953) (Experimental, Phase Diagram, Phase Relations, 17) Boehm, H., Westphal, H., “Transformation of β into α and ω in Titanium Alloys”, Z. Metallkd., 47, 558–563 (1956) (Morphology, Experimental, Phase Diagram, Phase Relations, Mechan. Prop., 6) Zwicker, U., “The Titan-Aluminium-Chromium and Titan-Aluminium-Vanadium Systems and Technical Alloys with 5% Cr and 3% Al Also 6% Al and 4% V” (in German), Z. Metallkd., 47, 535–548 (1956) (Experimental, Mechan. Prop., Phase Diagram, 12) Tagunova, T.V., “The Ti-Cr-Al System”, Zh. Neorg. Khim., 3, 815–819 (1958) (Experimental, Phase Diagram, Phase Relations, 3) Kornilov, I.I., Mikheev, V.S., Chernova, T.S., “Investigations of Phase Diagram of the Ti-Cr-Al System” (in Russian), Zh. Neorg. Khim., 3(3), 786–796 (1958) (Morphology, Experimental, Phase Diagram, Phase Relations, 6) Ence, E., Farrar, P.A., Margdin, H., “Binary and Ternary Diagrams of the Ti-Al-Cr and Ti-Al-V Systems”, Wright Air Develop. Division, Techn. Rep., 60–316 (1960) Zoller, H., “The Influence of Zinc, Magnesium, Silicon, Copper, Manganese, Titanium on the Primary Crystallization of Al7Cr” (in German), Schweizer Archiv, 478–491 (1960) (Experimental, Phase Diagram, 33) Luzhnikov, L.P., Novikova, V.M., Mareev, A.P., “Solubility of β Stabilisers in α-Ti”, Met. Sci. Heat Treat., 5(2), 78–81 (1963) translated from Metallov. Term. Obrab. Met., (2), 13–16 (1963) (Experimental, Phase Diagram, Phase Relations, 4) Weigand, H.H., “Transformation in α / β Ti Alloys Containing Al”, Z. Metallkd., 54, 43–49 (1963) (Experimental, Phase Relations, Morphology, 16) Raman, A., Schubert, K., “The Occurence of Zr2Cu- and Cr2Al-Type Intermetallic Compounds”, Z. Metallkd., 55, 798–804 (1964) (Experimental, 23) Schubert, K., Raman, A., Rossteutscher, W., “Structural Data of some Metallic Phases (10)” (in German), Naturwissenschaften, 51, 506–507 (1964) (Crys. Structure, 0) Zwicker, U., “Titanium and Titanium Alloys” (in German), Springer, Berlin, 576–585 (1974) (Phase Diagram, Phase Relations, Review, 300) Jacob, I., Shaltiel, D., “A Note on the Influence of Al on the Hydrogen Sorption Properties of Ti(AlxB1–x)2 (B = Cr, Mn, Fe, Co)”, Mater. Res. Bull., 13, 1193–1198 (1978) (Crys. Structure, Experimental, 10) Suprunenko, P.A., Markiv, V.Ya., Tsvetkova, T.M., “Magnetic and X-Ray Diffraction Study of Laves Phases in the Ternary Systems (Ti, Zr, Hf)-Cr-Al”, Russ. Metall., (1), 207–210 (1984) translated from Izv. Akad. Nauk SSSR, Metally, (1), 207–210 (1984) (Experimental, 11) Gros, J.P., Ansara, I., Allibert, M., “Prediction of α/β Equilibria in Titanium-Based Alloys Containing Al, Mo, Zr, Cr. II”, Les Editions de Physique. Avenue du Hoggar, Zone Industrielle de Courtaboeuf, B.P. 112, F-91944 Les Ulis Cedex, France. 1988; Accession Number: 90(9):72–359; Conference: Sixth World Conference on Titanium. III, Cannes, France, 6–9 June 1988, 1559–1564 (1988) (Phase Diagram, Phase Relations, 0) Kim, Y.-W., “Intermetallic Alloys Based on γ Titanium Aluminide”, JOM, 24–30 (1989) (Crys. Structure, Mechan. Prop., Phase Diagram, Phase Relations, Review, 61) Lampman, S., “Wrought Titanium and Titanium Alloys”, Metals Handbook, Tenth Edition. Vol. 2. Properties and Selection: Nonferrous Alloys and Special-Purpose Materials, 2, 592–633 (1990) (Experimental, Interface Phenomena, Mechan. Prop., Phase Diagram, 36) Mabuchi, N., Hirukawa, K., Tsuda, H., Nakayama, Y., “Formation of Structural L12 Compounds in the Ternary Al-Ti-Cr System”, Scr. Metall., 24(3), 505–508 (1990) (Crys. Structure, Experimental, 20) Zhang, S., Nic, J.P., Mikkola, D.E., “New Cubic Phases Formed by Alloying Al3Ti with Mn and Cr”, Scr. Metal. Mater., 24(1), 57–62 (1990) (Crys. Structure, Experimental, Mechan. Prop., 13)
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti [1991Bea]
[1991Dur]
[1991Hua]
[1991Mab]
[1991Mae] [1991Mas]
[1991Mik] [1991Moh] [1991Nic]
[1991Par]
[1991Spa]
[1992Dur] [1992Hay] [1992Kim]
[1992Miz] [1992Mor] [1992Nic]
[1992Win] [1992Zhe]
[1993Ers]
[1993Hao]
7
Beaven, P.A., Pfullmann, Th., Rogalla, J., Wagner, R., “Rhase Transformations and Microstructural Development in TiAl-Based Alloys”, Mater. Res. Soc. Symp. Proc.: High-Temp. Ordered Intermetallic Alloys IV, 213, 151–156 (1991) (Experimental, Phase Relations, 9) Durlu, N., Inal, O.U., Yost, F. G., “L1(2)-Type Ternary Titanium Aluminides of the Composition Ti25X8Al67: TiAl3-Based or TiAl2-Based?”, Scr. Metall. Mater., 25(11), 2475–2479 (1991) (Crys. Structure, Review, 30) Huang, S.C., Hall, E.L., Shih, D.S., “Microstructure and Ductility of TiAl Alloys Modified by Chromium Additions”, ISIJ Intl., 31(10), 1100–1105 (1991) (Electronic Structure, Experimental, Mechan. Prop., 17) Mabuchi, H., Nakayama, Y., “Development of Al-Ti-X Ternary L12 Intermetallic Compounds” (in Japanese), Bull. Jpn. Inst. Met., 30(1), 24–30 (1991) (Crys. Structure, Experimental, Mechan. Prop., Phase Diagram, 36) Maeda, T., Okada, M., Shida, Y., “Ductility and Strength in Mo Modified TiAl”, Mater. Res. Soc. Symp. Proc.: High-Temp. Ordered Intermetallic Alloys IV, 213, 555–560 (1991) (Experimental, Phys. Prop., 15) Masahashi, N., Mizuhara, Y., Matsuo, M., Hashimoto, K., Kimura, M., Hanamura, T., Fujii, H., “Ternary Alloying of γ Titanium-Aluminides for Hot-Workability”, Mater. Res. Soc. Symp. Proc.: HighTemp. Ordered Intermetallic Alloys IV, 213, 795–800 (1991) (Experimental, Phys. Prop., 9) Mikkola, D.E., Nic, J.P., Zhang, S., Milligan, W.W., “Alloying of Al3Ti to Form Cubic Phases”, ISIJ Intl., 31(10), 1076–1079 (1991) (Crys. Structure, Experimental, Mechan. Prop., 16) Mohandas, E., Beaven, P.A., “Site Occupation of Nb, V, Mn and Cr in γ-TiAl”, Scr. Metall. Mater., 25 (9), 2023–2027 (1991) (Crys. Structure, Experimental, 15) Nic, J.P., Zhang, S., Mikkola, D.E., “Alloying of Al3Ti with Mn and Cr to Form Cubic L12 Phases”, Mater. Res. Soc. Symp. Proc.: High-Temp. Ordered Intermetallic Alloys IV, 213, 697–702 (1991) (Crys. Structure, Experimental, Mechan. Prop., Phase Diagram, 12) Parfitt, L.J., Smialek, J.L., Nic, J.P., Mikkola, D.E., “Oxidation Behavior of Cubic Phases Formed by Alloying Al3Ti with Cr and Mn”, Scr. Metall. Mater., 25, 727–731 (1991) (Electrochem., Experimental, Phys. Prop., 11) Sparks, C.J., Porter, W.D., Schneibel, J H., Oliver, W.C., Golec, C.G., “Formation of Cubic L12 Phases from Aluminum Titanium (Al3Ti) and Aluminum Zirconium (Al3Ar) by Transition Metal Substitutions for Aluminum”, Mater. Res. Soc. Symp. Proc., 186, 175–80 (1991) (Crys. Structure, Experimental, 15) Durlu, N., Inal, O.T., “L12-Type Ternary Titanium Aluminides as Electron Concentration Phases”, J. Mater. Sci., 27(12), 3225–3230 (1992) (Assessment, Crys. Structure, 41) Hayes, F.H., “The Al-Cr-Ti System (Aluminum-Chromium-Titanium)”, J. Phase Equilib., 13(1), 79–86 (1992) (Crys. Structure, Phase Diagram, Phase Relations, Review, 90) Kimura, M., Hashimoto, K., Morikawa, H., “Study on Phase Stability in Ti-Al-X Systems at High Temperatures”, Mater. Sci. Eng. A, 152A(1–2), 54–59 (1992) (Abstract, Crys. Structure, Experimental, Phase Diagram, 12) Mizuhara, Y., Masahashi, N., “The Phase Stability of γ Titanium Aluminides with the β Phase”, Scr. Metall. Mater., 27, 1079–1084 (1992) (Experimental, Mechan. Prop., Morphology, 5) Morris, D.G., Gunter, S., “Ordering Ternary Atom Location and Ageing in Ll2 Trialuminide Alloys”, Acta Metall. Mater., 40(11), 3065–3073 (1992) (Experimental, 23) Nic, J.P., Klansky, J.L., Mikkola, D.E., “Structure/Property Observations for Al-Ti-Cr Alloys Near the Cubic (Al,Cr)3Ti Phase”, Mater. Sci. Eng. A, 152(1/2), 132–137 (1992) (Crys. Structure, Experimental, Mechan. Prop., Phase Diagram, 16) Winnicka, M.B., Varin, R.A., “Microstructure and Ordering of L12 Titanium Trialuminides”, Metall. Trans. A, 23A(11), 2963–2972 (1992) (Crys.Structure, Experimental, Morphology, 24) Zheng, Y., Zhao, L., Tangri, K., “Microstructure Evolution During Heat Treatment of a ChromiumBearing Ti3Al + TiAl Alloy”, Scr. Metall. Mater., 26(2), 219–224 (1992) (Experimental, Mechan. Prop., Morphology, 19) Erschbaumer, H., Podloucky, R., Rogl, P., Temnitschka, G., Wagner, R., “Atomic Modelling of Nb, V, Cr and Mn Substitutions in γ-TiAl. I: c/a Ratio and Site Preference”, Intermetallics, 1, 99–106 (1993) (Calculation, Crys. Structure, 31) Hao, S.M., Liu, X.J., Zheng, Z.Z., Zeng, N.H., “A Study on the Isothermal Section of Phase Diagram in Ti-Al-Cr System at 1000˚C”, Proc. 7th Nat. Symp. Phase Diagrams, 14–16 (1993) (Experimental, Phase Diagram, 0)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
41
42
7 [1993Has]
[1993Kaw]
[1993Nak] [1993Wri]
[1994Boh]
[1994Gao] [1994Kla] [1994Li]
[1994Sok]
[1994Zha] [1994Zhe] [1995Bra] [1995Jew] [1995Hao]
[1995Kog] [1995Nak] [1995Whi]
[1996Jew1] [1996Jew2] [1996Jew3] [1996Liu]
[1996Woo]
Al–Cr–Ti Hashimoto, K., Masao, K., “Effects of Third Element Addition on Mechanical Properties of TiAl”, Struct. Intermet.: 1st Int. Symp. Struct. Intermetallics, Champion Pa. Sept., The Miner., Mater. and Mater. Soc., Daralia, R., Lewandowski, J.J., Liu, C.T., Martin, P.L., Mirakle, D.B., Nathal, M.V. (Eds.), 309–318 (1993) (Experimental, Mechan. Prop., Phase Diagram, 18) Kawabata, T., Tamura, T., Izumi, O., “Effect of Ti/Al Ratio and Chromium, Niobium, and Hafnium Additions on Material Factors and Mechanical Properties in TiAl”, Metall. Trans. A, 24(1), 141–150 (1993) (Crys. Structure, Experimental, Mechan. Prop., 20) Nakayama, Y., Mabuchi, H., “Formation of Ternary L12 Compounds in Al3Ti-Base Alloys”, Intermetallics, 1, 41–48 (1993) (Crys. Structure, Experimental, Mechan. Prop., Phase Diagram, 40) Wright, R.N., Erickson, A.E., O’Brien, M.H., Rabin, B.H., “Characterization of Al2Ti Precipitates in Cubic Al64.5Ti27.5Cr8”, Scr. Metall. Mater., 28(10), 1293–1297 (1993) (Electronic Structure, Experimental, Mechan. Prop., 19) Bohnenkamp, U., Wang, G.-X., Jewett, T.J., Dahms, M., “A Quantitative Investigation of Phase Formation During Annealing of Cold-Extruded Elemental Powder Mixtures Ti-48 at.% Al and Ti-48 at.% Al-2 at.% Cr”, Intermetallics, 2, 275–283 (1994) (Crys. Structure, Experimental, Phase Diagram, Thermodyn., 20) Gao Y., Zhu J., Cai Q.G., “Microstructure of the Ordered β Phase in Ti-Al Alloy with Chromium and Vanadium.”, Scr. Met. Mater., 31(5), 571–575 (1994) (Experimental, Morphology, 12) Klansky, J.I., Nic, J.P., Mikkola, D.E., “Structure/Property Observations for Al-Ti-Cr Intermetallic Alloys”, J. Mater. Res., 9(2), 255–258 (1994) (Crys. Structure, Experimental, Phase Diagram, 13) Li, Y.G., Loretto, M.H., “Microstructure and Fracture Behaviuor of Ti-44Al-xM Derivatives”, Acta Metall. Mater., 42(9), 2913–2919 (1994) (Crys. Structure, Experimental, Mechan. Prop., Phase Relations, 12) Sokolovskaya, E.M., Kazakova, E.F., Poddyakova, E.I., Portnoi, V.K., Temirbaeva, A.A., “Phase Composition of Alloys of the Al-Cr-Ti System at 770 K” (in Russian), Vestn. Mosk. Univ. Ser. 2: Khim., 35(5), 453–454 (1994) (Phase Diagram, Phase Relations, Experimental, 5) Zhang, B., Wang, J., Wan, X., Chen, W., “A Study on the β and ω Phases in a Ti-Al-Cr Alloy”, Scr. Metall. Mater., 30, 399–404 (1994) (Crys. Structure, Experimental, 13) Zhang, J.G., Li, Q., Liu, Z.G., Feng, D., Frommeyer, G., “Complex Stacking Fault Energy of Cr-Alloyed γ-TiAl”, Phys. Lett. A, 196, 125–127 (1994) (Crys. Structure, Experimental, 11) Brady, M.P., Smialek, J.L., Terepka, F., “Microstructure of Alumina-Forming Oxidation Resistant AlTi-Cr Alloys”, Scr. Metall. Mater., 32(10), 1659–1664 (1995) (Experimental, Phase Relations, 17) Jewett, T.J., Dahms, M., “Investigation of the γ-Ti(Cr,Al)2 Phase at 800˚C and 1000˚C”, Scr. Metall. Mater., 32(10), 1533–1539 (1995) (Experimental, Phase Relations, 18) Hao, S., Zeng, L., “Isothermal Section of Phase Diagram in Ti-Al-Cr Ternary System at 1000˚C”, Acta Metall. Sin. (China), 31(4), B152-B158 (1995) (Experimental, Morphology, Phase Diagram, Phase Relations, 5) Kogachi, M., Kameyama, A., “Composition Dependence of site Occupancies in Ternary L12 Compound Al3Ti-Cr”, Intermetallics, 3, 327–334 (1995) (Crys. Structure, Experimental, 29) Nakai, K., Ono, T., Ohtsubo, H., Ohmori, Y., “Phase Stability and Decomposition Processes in Ti-Al Based Intermetallics”, Mater. Sci. Eng. A, 192-193, 922–929 (1995) (Experimental, Phase Relations, 21) Whittenberger, J.D., Kumar, K.S., DiPietro, M.S., Brown, S.A., “Characteristics of Elevated Temperature Deformation in Several L12-Modified Al3Ti-Based Alloys”, Intermetallics, 3, 221–232 (1995) (Experimental, Mechan. Prop., 32) Jewett, T., Dahms, M., “Stability of the Ti(Cr,Al)2 Phase”, Z. Metallkd., 87(4), 254–261 (1996) (Crys. Structure, Experimental, Mechan. Prop., Phase Relations, 33) Jewett, T.J., Ahrens, B., Dahms, M., “Phase Equlibria Involting the τ-L12 and TiAl2 Phases in the Ti-AlCr System”, Intermetallics, 4, 543–556 (1996) (Experimental, Phase Relations, 31) Jewett, T.J., Ahrens, B., Dahms, M., “Stability of the L12 Phase at 800˚C C in the Ti-Al-Cr-System”, Scr. Mater., 34(3), 395–399 (1996) (Crys. Structure, Experimental, Mechan. Prop., Morphology, 13) Liu, S., Hu, R., Zhao, D., Wang, C., Luo, P., Pu, Z., “Bonding Characteristics of the Intermetallic Compound Al3Ti+Cr”, J. Mater. Sci. Technol., 12, 180–184 (1996) (Crys. Structure, Electronic Structure, Experimental, 30) Woodward, C., MacLaren, J.M., “Planar Fault Energies and Sessile Dislocation Configurations in Substitutionally Disordered Ti-Al with Nb and Cr Ternaty Additions”, Philos. Mag. A, 74(2), 337–357 (1996) (Calculation, Crys. Structure, 43)
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti [1997Jew] [1997Fan] [1997Hei] [1997Mab1]
[1997Mab2]
[1997Mas] [1997Ley]
[1997Par]
[1997Xu] [1998Jim]
[1998Jun]
[1998Has] [1999Yan]
[1999Jac] [1999Hao] [1999Nic] [1999Sha] [1999Yam]
[2000Cha]
[2000Coe]
[2000Kai1]
7
Jewett, T.J., Ahrens, B., Dahms, M., “Stability of TiAl in the Ti-Al-Cr System”, Mater. Sci. Eng. A, 225, 29–37 (1997) (Crys. Structure, Experimental, Phase Relations, 26) Fan, G.J., Song, X.P., Quan, M.X., Hu, Z.Q., “Mechanical Alloying and Thermal Stability of Al67Ti25M8 (M = Cr,Zr,Cu)”, Mater. Sci. Eng. A, 231, 111–116 (1997) (Crys. Structure, Experimental, 22) Heilmaier, M., Saage, H., Eckert, J., “Formation of ODS L12-(Al, Cr)3Ti by Mechanical Alloying”, Mater. Sci. Eng. A, 239-240, 652–657 (1997) (Experimental, Mechan. Prop., 18) Mabuchi, H., Tsuda, H., Matsui, T., Morii, K., “185. Microstructure and Mechanical Properties of Ternary L12 Intermetallic Compound in Al-Ti-Cr System”, Metall. Abstr. Light Met. Alloys, 30, 208–210 (1996-1997) (Experimental, Phase Diagram, Phase Relations, 0) Mabuchi, H., Tsuda, H., Matsui, T., Morii, K., “Microstructure and Mechanical Properties of Ternary L12 Intermetallic Compound in Al-Ti-Cr System”, Mater. Trans., JIM, 38(6), 560–565 (1997) (Crys. Structure, Experimental, Mechan. Prop., Phase Relations, 40) Masahashi, N., Mizuhara, Y., “APFIM Study of β and γ Microduplex TiAl Intermetallic Alloys”, Mater. Sci. Eng. A, 223, 29–35 (1997) (Experimental, Phys. Prop., 24) Leyens, C., Schmidt, M., Peters, M., Kaysser, W.A., “Sputtered Intermetallic Ti-Al-X Coatings: Phase Formation and Oxidation Behavior”, Mater. Sci. Eng. A, 239-240, 680–687 (1997) (Experimental, Morphology, 17) Park, J.Y., Oh, M.H., Wee, D.M., Miura, S., Mishima, Y., “L12 (Al,Cr)3Ti-Based Two-Phase Intermetallic Compounds-I. Plastic Deformation Behavior”, Scr. Mater., 36(7), 795–800 (1997) (Experimental, Phase Relations, 12) Xu, H., Jin, Z., Wang, R., “Study of the Phase Equilibria of Al-Cr-Ti System at 1050˚C”, Scr. Mater., 37(10), 1469–1473 (1997) (Experimental, Phase Relations, 25) Jimenez, J.A., Wesemann, J., Frommeyer, G., “High-Temperature Deformation Behavior of the Intermetallic Ti-47 at.% Al-3 at.% Cr Alloy”, Metall. Mater. Trans. A, 29, 1425–1430 (1998) (Electronic Structure, Experimental, Mechan. Prop., 29) Jung, J.Y., Park, J.K., “Growth Kinetics of Discontinous Coarsening of Lamellar Structure in Ti-44 at.% Al (-0.5 at.% Cr) Intermetallic Compounds”, Acta Mater., 46(12), 4123–4130 (1998) (Crys. Structure, Experimental, Kinetics, Thermodyn., 31) Hashimoto, K., Kimura, M., Mizuhara, Y., “Alloy Design of γ Titanium Aluminides Based on Phase Diagrams”, Intermetallics, 6, 667–672 (1998) (Experimental, Phase Relations, 14) Yang, R., Hao, Y.L., “Estimation of (γ + α2) Equilibrium in Two-Phase Ti-Al-X Alloys by Means of Sublattice Site Occupancies of x in TiAl and Ti3Al”, Scr. Mater., 41(3), 341–346 (1999) (Calculation, Phase Relations, 13) Jacobson, N.S., Brady, M.P., Mehrotra, G.M., “Thermodynamics of Selected Ti-Al and Ti-Al-Cr Alloys”, Oxid. Met., 52(5/6), 537–556 (1999) (Experimental, Phase Relations, Thermodyn., 48) Hao, Y.L., Xu, D.S., Cui, Y.Y., Yang, R., Li, D., “The Site Occupancies of Alloying Elements in TiAl and Ti3Al Alloys”, Acta Mater., 47(4), 1129–1139 (1999) (Crys. Structure, Experimental, 41) Nic, J.P., Mikkola, D.E., “Site Occupancy in Ternary L12 Ordered Alloys as Determined by Diffarction: Observations on (Al,Cr)3Ti Alloys”, Intermetallics, 7, 39–47 (1999) (Crys. Structure, Experimental, 20) Shao, G., Tsakiropoulos, P., “Solidification Structures of Ti-Al-Cr Alloys”, Intermetallics, 7, 579–587 (1999) (Experimental, Phase Relations, 15) Yamamoto, Y., Hashimoto, K., Kimura, T., Nobuki, M., Kohno, N., “L12 Single Phase Region in Al-Ti Base Ternary and Quaternary Systems at 1450 K” (in Japanese), J. Jpn. Inst. Met., 63(10), 1317–1326 (1999) (Crys. Structure, Experimental, Phase Relations, 15) Chatterjee, A., Dehm, G., Scheu, C., Clemens, H., “Onset of Microstructural Instability in a Fully Lamellar Ti-46.5 at.% Al-4 at.% (Cr,Nb,Ta,B) Alloy During Short-term Creep”, Z. Metallkd., 91 (9), 755–760 (2000) (Experimental, Mechan. Prop., Phase Relations, 21) Coelho, C., Ramos, A.S., Trindade, B., Vieira, M.T., Fernandes, J.V., Vieira, M., “Characterisation of Modified Sputtered (TiAl)-Based Intermetallic Materials Doped with Silver and Chromium”, Key Eng. Mater., 188, 37–44 (2000) (Experimental, Mechan. Prop., 13) Kainuma, R., Ohnuma, I., Ishukawa, K., Ishida, K., “Stability of B2 Ordered Phase in the Ti rich Portion of Ti-Al-Cr and Ti-Al-Fe Ternary Systems”, Intermetallics, 8, 869–875 (2000) (Crys. Structure, Experimental, Phase Relations, 19)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
43
44
7 [2000Kai2]
[2000Mab]
[2000Ohi]
[2000Sha] [2000Wel] [2000Yan]
[2000Zhu] [2001Ich]
[2001Ish]
[2001Fuj]
[2001Kan]
[2001Kau] [2001Lee]
[2001Mil]
[2001Mor] [2001Sun]
[2001Sur] [2001Xia]
[2001Yam]
[2001Zho]
Al–Cr–Ti Kainuma, R., Fujita, Y., Mitsui, H., Ishida, K., “Phase Equilibria Among α (hcp), β (bcc) and γ (L10) Phases in Ti-Al Base Ternary Alloys”, Intermetallics, 8, 855–867 (2000) (Crys. Structure, Experimental, Phase Relations, 29) Mabuchi, H., Tsuda, H., Matsui, T., Morii, K., “Effects of Vanadium Addition on the Material Properties of L12-Type Ordered Alloys in the Al-Ti-Cr System”, J. Jpn. Inst. Met., 64(11), 1041–1047 (2000) (Crys. Structure, Experimental, Phase Relations, 39) Oh-ishi, K., Kumamoto, H., Horita, Z., Nemoto, M., “Phase Separation in TiAl(L10)-(Al,Cr)3Ti(L12) System” (in Japanese), J. Jpn. Inst. Met., 64(8), 609–615 (2000) (Experimental, Mechan. Prop., Phase Relations, 14) Shao, G., Tsakiropoulos, P., “On the w Phase Formation in Cr-Al and Ti-Al-Cr Alloys”, Acta Mater., 48, 3671–3685 (2000) (Calculation, Crys. Structure, Experimental, Phase Relations, 39) Weller, M., Chatterjee, A., Haneczok, G., Clemens, H., “Internal Friction of γ-TiAl Alloys at High Temperature”, J. Alloys Compd., 310, 134–138 (2000) (Experimental, Mechan. Prop., 15) Yang, R., Hao, Y., Song, Y., Guo, Z.X., “Site Occupancy of Alloying Additions in Titanium Aluminides and its Application to Phase Equilibrium Evaluation”, Z. Metallkd., 91(4), 296–301 (2000) (Crys. Structure, Phase Relations, Review, 38) Zhuang, W., Shen, J., Liu, Y., Shang, S., Du, Y., Schuster J.C., “Thermodynamic Optimisation of the Cr-Ti System”, Z. Metallkd., 91, 121–127 (2000) (Thermodyn., Phase Diagram, 53) Ichimaru, M., Mori, N., Miura, Y., “Al-Ti-Cr Ternary Phase Diagram and Solidification Structure of (Al,Cr)3Ti Alloys”, J. Jpn. Inst. Light Met., 51(12), 640–645 (2001) (Experimental, Morphology, Phase Diagram, Phase Relations, 9) Ishikawa, K., Hashi, K., Suzuki, K., Aoki, K., “Effect of Substitutional Elements on the Hydrogen Absorption-Desorption Properties of Ti3Al Compounds”, J. Alloys Compd., 314, 257–261 (2001) (Experimental, Phase Relations, 9) Fujita, T., Ikeda, H., Tanaka, S., Horita, Z., “Construction of Ti-Al-Cr Phase Diagram Using Quantitative X-Ray Microanalysis in Analytical Electron Microscope” (in Japanese), J. Jpn. Inst. Met., 65(5), 382–388 (2001) (Crys. Structure, Experimental, Phase Relations, 20) Kang, S.Y., Onodera, H., “Analyses of HCP/D019 and D019/L10 Phase Boundaries in Ti-Al-X (X = V, Mn, Nb, Cr, Mo, Ni and Co) Systems by the Cluster Variation Method”, J. Phase Equilib., 22, 424–430 (2001) (Calculation, Phase Relations, 15) Kaufman, L., “Calculation of Multicomponent Phase Diagrams for Niobium Alloys”, Niob. Sci. Tech., 107–120 (2002) (Calculation, Phase Diagram, 20) Lee, C.Y., Park, J.K., “Effect of Cr and Si Additions on the Continuous-Cooling-Transformation Kinetics of γ-Based Ti-45 at.% Al Alloy”, Philos. Mag. A, 81(10), 2415–2426 (2001) (Crys. Structure, Experimental, Kinetics, 14) Milman, Yu.V., Miracle, D.B., Chugunova, S.I., Voskoboinik, I.V., Korzhova, N.P., Legkaya, T.N., Podrezov, Yu.N., “Mechanical Behaviour of Al3Ti Intermetallic and L12 Phases on Its Basis”, Intermetallics, 9, 839–845 (2001) (Crys. Structure, Experimental, Mechan. Prop., 36) Mori, N., Ogi, K., “Analisis of Solidification-Path of Al-Ti-Cr Alloys by Progressive-Type Solidification Equations” (in Japanese), J. Jpn. Inst. Met., 65(9), 848–851 (2001) (Experimental, Phase Relations, 12) Sun, F.-S., Cao, C.-X., Kim, S.-E., Lee, Y.-T., Yan, M.-G., “Alloying Mechanism of β Stabilizers in a TiAl Alloy”, Metall. Mater. Trans. A, 32A, 1573–1589 (2001) (Crys. Structure, Experimental, Mechan. Prop., Phase Relations, 37) Suryanarayana, C., “Mechanical Alloying and Milling”, Prog. Mater. Sci., 46(1-2), 1–184 (2001) (Crys. Structure, Experimental, Kinetics, Phase Relations, Review, Thermodyn., 932) Xia, Q., Wang, J.N., Yang, J., Wang, Y., “On the Massive Transformation in TiAl-based Alloys”, Intermetallics, 9, 361–367 (2001) (Crys. Structure, Experimental, Mechan. Prop., Phase Relations, Thermodyn., 29) Yamamoto, Y., Hashimoto, K., Kimura, T., Nakamura, M., Kohno, N., “Residual Strain in Mechanically Ground Powders of Al-Ti Base Ternary and Quaternary Compounds with Ll2 Single-Phase at 1450K”, Mater. Trans., JIM, 42(7), 1392–1399 (2001) (Crys. Structure, Experimental, Phase Relations, 18) Zhou, Ch., Yang, Y., Gong, Sh., Xu, H., “Effect of Ti-Al-Cr Coatings on the High Temperature Oxidation Behavior of TiAl Alloys”, Mater. Sci. Eng. A, 307, 182–187 (2001) (Crys. Structure, Experimental, Kinetics, 13)
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Cr–Ti [2002Bra]
[2002Cal]
[2003Bar]
[2003Lee]
[2003Mor]
[2003Nis1] [2003Nis2]
[2003Ram] [2003Zha] [2004Nay] [2004Wan] [2005App] [2005Rag] [2006Fox]
[2006Nar]
[2006Sch] [2007Hes]
[2007Wit]
[2008Cor]
[2008Iva]
7
Brandt, C., Inal, O. T., “Mechanical Properties of Cr, Mn, Fe, Co, and Ni Modified Titanium Trialuminides”, J. Mater. Sci., 37(20), 4399–4403 (2002) (Crys. Structure, Experimental, Mechan. Prop., 17) Calderon, H.A., Garibay-Febles, V., Umemoto, M., Yamaguchi, M., “Mechanical Properties of Nanocrystalline Ti-Al-X Alloys”, Mater. Sci. Eng. A, 329-331, 196–205 (2002) (Experimental, Mechan. Prop., Morphology, 26) Barabash, O.M., Milman, Yu.V., Miracle, D.V., Karpets, M.V., Korzhova, N.P., Legkaya, T.N., Mordovets, N.M., Podrezov, Yu.N., Voskoboinik, I.V., “Formation of Periodic Mecrostructures Involving the L12 Phase in Eutectic Al-Ti-Cr Alloys”, Intermetallics, 11(9), 953–962 (2003) (Crys. Structure, Experimental, Mechan. Prop., Phase Diagram, 26) Lee, J.K., Oh, M.W., Oh, M.H., Wee, D.M., “Phase Stability of L12-Based Alloys in Al-Ti-Cr Systems”, Intermetallics, 11(8), 857–865 (2003) (Crys. Structure, Experimental, Mechan. Prop., Morphology, Phase Relations, 24) Mori, N., Ogi, K., “Solidification-Path and Microstructure of Al-Ti-Cr Alloy Analyzed by ProgressiveType Solidification Equation”, Mater. Trans., JIM, 44(11), 2334–2338 (2003) (Calculation, Phase Relations, 15) Nishimoto, T., Izumi, T., Hayashi, S., Narita, T., “Two-Step Cr and Al Diffusion Coating on TiAl at High Temperatures”, Intermetallics, 11, 225–235 (2003) (Experimental, Transport Phenomena, 38) Nishimoto, T., Izumi, T., Hayashi, Sh., Narita, T., “Effect of Coating Layer Structures and Surface Treatments on the Oxidation Behavior of a Ti-50 at.% Al Alloy”, Intermetallics, 11(5), 459–466 (2003) (Experimental, Interface Phenomena, Kinetics, Mechan. Prop., 46) Ramos, A.S., Vieira, M.T., “Properties of γ-TiAl-M (M=Ag, Cr) Sputtered Films”, Mater. Sci. Forum, 426-432, 1843–1848 (2003) (Electronic Structure, Experimental, Mechan. Prop., 20) Zhang, W.J., Deevi, S.C., “The Controlling Factor in Primary Creep of TiAl-Based Alloys”, Intermetallics, 11(2), 177–185 (2002) (Experimental, Mechan. Prop., 34) Nayak, S.S., Murty, B.S., “Synthesis and Stability of L12-Al3Ti by Mechanical Alloying”, Mater. Sci. Eng. A, 367(1-2), 218–224 (2004) (Crys. Structure, Experimental, Morphology, Phase Relations, 25) Wang, Y., Wang, J.N., Yang, J., “Superplastic Behavior of a High-Cr TiAl Alloy in its Cast State”, J. Alloys Compd., 364(1-2), 93–98 (2004) (Experimental, Mechan. Prop., 10) Appel, F., “An Electron Microscope Study of Mechanical Twinning and Fracture in TiAl Alloys”, Philos. Mag., 85(2-3), 205–231 (2005) (Experimental, Mechan. Prop., Morphology, Phase Relations, 74) Raghavan, V., “Al-Cr-Ti (Aluminum-Cromium-Titanium)”, J. Phase Equilib. Diffus., 26, 349–356 (2005) (Review, Phase Diagram, 35) Fox-Rabinovich, G.S., Wilkinson, D.S., Veldhuis, S.C., Dosbaeva, G.K., Weatherly, G.C, “Oxidation Resistant Ti-Al-Cr Alloy for Protective Coating Applications”, Intermetallics, 14(2), 189–197 (2006) (Crys. Structure, Experimental, Interface Phenomena, Kinetics, Morphology, Phase Relations, 20) Narita, T., Izumi, T., Nishimoto, T., Shibata, Y., Thosin, K.Z., Hayashi, S., “Advanced Coatings on High Temperature Applications”, Mater. Sci. Forum, 522-523, 1–14 (2006) (Phase Diagram, Phase Relations, Review, 15) Schuster, C., Palm, M., “Reassessment of the Binary Aluminium-Titanium Phase Diagram”, J. Phase Equilib. Diffus., 27(3), 255–277 (2006) (Review, Phase Diagram, Crys. Structure, 375) Heshmanu-Manesh, S., Ahmadabadi, M.N., Ghasemiarmaki, H., Jafarian. H.R., “Effect of Initial Microstructure and Further Thermomechanical Processing on Microstructural Evolution in a Ti-47Al2Cr Alloy”, J. Alloys Compd., 436, 200–203 (2007) (Experimental, Morphology, 10) Witusiewicz, V.T., Bondar, A.A., Hecht, U., Rex, S., Velikanova, T.Ya., “The Al-B-Nb-Ti System. III. Thermodynamic Re-Evaluation of the Constituent Binary System Al-Ti”, in press, J. Alloys Compd., DOI:10.1016/j.jallcom.2007.10.061 (2007) (Phase Relations, Phase Diagram, Experimental, Thermodyn., Calculation, Review, 89) Cornish, L., Saltykov, P., Cacciamani, G., Velikanova, T., “Al-Cr (Aluminium-Cromium), MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; to be published, (2008) (Phase Diagram, Crys. Structure, Thermodyn., Assessment, 51) Ivanchenko, V., “Cr-Ti (Chromium-Titanium)”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; to be published, (2008) (Phase Diagram, Crys. Structure, Thermodyn., Assessment, 22)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
45
46
7 [Mas2] [V-C2]
Al–Cr–Ti Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
DOI: 10.1007/978-3-540-88053-0_7 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
Aluminium – Iron – Niobium Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Sergio Gama, updated by Annelies Malfliet
Introduction [1966Ram] first reported an isothermal section at 1000˚C, followed by [1970Bur] who provided an 800˚C isotherm. There is reasonable agreement between the two works. Interestingly, however, both investigators found a ternary phase, called μ’, although the position and solubility range of this phase is drawn differently in both sections. Some diffraction lines of this phase are equal to those of the μ phase, but the exact crystal structure is unknown and further investigation is required. No other ternary phases were identified. More recently, a new version of the isothermal section at 1000˚C according to [1993Bej2] was presented in [1999Mot]. By comparing this section with the previous section at this temperature of [1966Ram], the μ’ phase is not present, while a new ternary Nb rich phase is observed. [1987Rag] provided a critical evaluation of the Al-Fe-Nb system, presenting a 800˚C isothermal section based on both [1966Ram] and [1970Bur], but containing the metastable Nb3Fe2 phase not considered by the former investigators. In the previous MSIT evaluation of [1992Gam] the isothermal section at 1000˚C determined by [1966Ram] is redrawn to be consistent with the accepted binaries. The Al-Fe-Nb system is also part of the review by [1990Kum] who highlights the inconsistencies in different studies of ternary Al-refractory metal-X systems. Most investigations on the applications of Al-Fe-Nb alloys are restricted to two composition regions. First, compositions around Fe-25Al with small percentages of Nb have been studied to improve the mechanical properties of this intermetallic through the formation of a two-phase microstructure of Fe3Al and λ, Nb(Fe1–xAlx)2, [1991Ran, 1997Par, 1999Den, 2004Mor2, 2005Mor, 2005Mot]. Secondly, Al-rich compositions are of interest due to the possibility to prepare nanocomposites with an amorphous matrix containing metallic nanocrystals through rapid quenching followed by the proper heat treatment. Investigations regarding the phase relations, structures and thermodynamics of the Al-Fe-Nb system are summarized in Table 1.
Binary Systems The Al-Fe system is accepted from [2006MSIT] which is mainly based on [1993Kat], except for the Fe rich corner, where the data of [2001Ike] are taken. For the Al-Nb system, the liquidus has not yet been fully determined and some inconsistencies in the invariant temperatures can be found by comparing different experimental studies. The accepted phase diagram is from [Mas2], mainly based on the work of [1980Jor], except for the Al-rich side which is based on [1966Lun]. The Fe-Nb system, presented in Fig. 1, is accepted from [1993Bej1]. This diagram Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
1
2
8
Al–Fe–Nb
is based on earlier work of the same author [1991Bej], where Nb3Fe2 is observed as a metastable phase around 61 at.% Nb.
Solid Phases The binary phases are described in Table 2. None of the Al-Fe binary compounds have appreciable solubility of Nb. For the Fe3Al phase, a solubility of 1 and 2 at.% Nb at 1300˚C is reported by respectively [2004Mor2] and [1988Dim], 1.6 at.% at 1150˚C by [2003Ste], 1 and 0.87 at.% at 1000˚C by respectively [1988Dim] and [2003Ste] and 0.5 at.% at 700˚C by [1988Dim]. For the binary Al-Nb phases, about 10 at.% Fe substitutes either Al or Nb in the σNb2Al phase at 1000˚C [1966Ram] and 2 at.% at 800˚C [1970Bur]. The NbAl3 phase takes up only little amount of Fe at 1000˚C [1966Ram]. The solubility range of this phase drawn at 5 at. % Fe in the preliminary study of [1966Ram], leads to the suggestion of [1989Sub] that Fe substitutes for Nb in the latter phase although no clear experimental details are given to validate this. For the Fe-Nb phases, a solubility of about 20 and 50 at.% Al in respectively μ, Nb19(Fe1–xAlx)21 and λ, Nb(Fe1–xAlx)2, at 1000˚C is found by [1966Ram]. This large solubility in both phases, whereby Al mainly substitutes for the Fe atoms, is confirmed in the investigation of the ternary system by [1970Bur] at 800˚C, reported as 26 at.% Al in μ, Nb19(Fe1–xAlx)21 and 56 at.% Al in λ, Nb(Fe1–xAlx)2. However, [1986Bla] concludes based on diffraction intensities of NbxFe2Al1–x alloys, that Al replaces the Nb atoms at the 8f positions in the hexagonal λ, Nb(Fe1–xAlx)2, phase, thereby replacing up to half the Nb atoms. [1966Ram] was the first to describe a ternary phase, called μ’, with basic stoichiometry Nb2FeAl existing in alloys kept for 168 h at 1000˚C. Most diffraction lines are equal to those of the μ, Nb19(Fe1–xAlx)21 phase, but some important ones are missing and new ones are observed. Although this indicates that μ’ is structurally related to the μ phase, the exact crystal structure is undetermined. [1970Bur] claims to observe this μ’ phase also in water quenched alloys kept for 1000 h at 800˚C, albeit at a different composition range than [1966Ram]. Therefore, as [1990Kum] states, it is not clear whether the same phase is observed in both investigations. In addition, the μ’ phase is completely absent in the isothermal section at 1000˚C of [1993Bej2] and as the solubility of the μ phase is extended to 27 at.% Al, this could indicate the metastable formation of the μ’ phase as observed by [1966Ram] from the μ phase. [1993Bej2] also observed a new ternary phase containing 5–10 at.% Fe and 19–25 at.% Al, but no crystallographic data are available.
Liquidus, Solidus and Solvus Surfaces Based on the substitution of Fe by Al in both λ, Nb(Fe1–xAlx)2, and FeAl, it is suggested in [1999Mot] that the eutectic valley between these phases should also follow a line of constant Nb. For Al-Fe-Nb alloys with 22.8, 41.2 and 45.0 at.% Al, the eutectic composition has been determined to contain respectively 9.7, 9.1 and 8.0 at.% Nb. Based on these measurements, a possible liquidus in this region of the phase diagram is constructed in Fig. 2. [2005Mot] found in addition that the coupled zone below the eutectic line is asymmetrically situated towards the λ, Nb(Fe1–xAlx)2, phase as a film of FeAl surrounds the primary λ, Nb(Fe1–xAlx)2, dendrites DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
in a hypereutectic alloy, while no λ, Nb(Fe1–xAlx)2, film surrounds the FeAl primary phase in a hypoeutectic alloy.
Isothermal Sections Two isothermal sections of the Al-Fe-Nb system are proposed by [1966Ram] and [1970Bur] at respectively 1000 and 800˚C, mainly based on metallographic and X-ray techniques. By comparing the two isothermal sections which differ only by 200˚C, two remarks should be mentioned. First, there is a significant difference in solubility of Fe in the binary Al-Nb phases. Secondly, the position and solubility range of the ternary μ’ phase in both sections is different. In his review, [1990Kum] poses the question whether these two μ’ phases are the same or different phases and states that further investigation of this part of the ternary system is recommended. [1987Rag] proposed an isothermal section at 800˚C based on both the results of [1966Ram] and [1970Bur] with the Al-Fe, Al-Nb and Fe-Nb binaries of respectively [1982Kub], [1981Ell] and [1982Kub]. In this combined section, a mean solubility of 5 at.% Fe in σ (Nb2Al) was assumed and the position of the μ’ phase was taken from [1970Bur]. To be in agreement with the binary Fe-Nb from [1982Kub], the metastable Nb3Fe2 phase was added. In [1999Mot] a more recent version of the isothermal section at 1000˚C as determined by [1993Bej2] is presented. This section is similar to the section proposed by [1966Ram] except for the region around μ’ and the ternary τ phase. The 1000˚C isothermal section presented in Fig. 3 is mainly taken from [1999Mot] as determined by [1993Bej2]. This section is preferred with respect to [1966Ram] as the latter only aimed for a rough estimation of the phase diagram by using metallographic and XRD techniques. Although no detailed information is available about the experimental work of [1993Bej2], from other works of this author in the same period [1991Bej, 1993Bej1, 1999Mot] it is known that this author had at least the opportunity to perform electron microprobe analysis to have a more precise composition analysis. In Fig. 4, the extension of the λ, Nb (Fe1–xAlx)2, phase in the two-phase region λ+FeAl is adjusted to the experimental results from [1988Dim]. The latter homogenized a Nb2Fe73Al25 alloy for 168 h at 1000˚C and found a twophase microstructure with 1Nb-74Fe-25Al (at.%) as the composition for the matrix and 25Nb-56Fe-19Al (at.%) as the composition for the λ, Nb(Fe1–xAlx)2 particles. [2004Mor2] confirmed that at high temperature the composition of the binary λ, NbFe2 phase in equilibrium with Fe3Al is close to NbFe3 and through the steady substitution of Fe by Al in the ternary system it evolves towards NbAl3. Figure 4 shows the isothermal section at 800˚C after [1970Bur], with some additional lines in the Al corner based on the binary systems.
Thermodynamics Thermodynamic data of the Al-Fe-Nb system are reported in Table 3. [1971Dub] used isothermal calorimetry based on an aluminothermic reaction to determine the heat of solution of aluminium in Fe-Nb alloys. The heat of solution is 105 ± 13 kJ·mol–1 for 1.3–6.3 mass% Al in a Fe-38.2Nb alloy and 100 ± 13 kJ·mol–1 for 1.9–9.5 mass% Al in a Fe-67.6Nb alloy. [2001Sud] used calorimetric data to estimate the enthalpy of mixing in the ternary Al-Fe-Nb system. Their calculations show that the addition of aluminium to Fe-Nb results in a minimum of the mixing enthalpy between –25 and –20 kJ·mol–1 located at the binary Al-Fe. Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
3
4
8
Al–Fe–Nb
Notes on Materials Properties and Applications Hardness tests have been performed on Nb1–xFe2Alx by [1986Bla] and on Nb33.4Fe33.6Al33.0 by [1996Mac]. According to [1962Min], the addition of Nb increases the hardness, electrical resistivity and improves the high temperature mechanical properties of the Fe3Al phase.The temperature dependence of the hardness of Nb2Fe68Al30, Nb2Fe73Al25, Nb5Fe75Al20 and Nb2Fe83Al15 has been measured by [2006Mor1, 2006Mor2]. The hardening is related to the change in state of order and, in particular, to the formation of a two-phase D03 order-plusdisorder microstructure. Above the temperature for onset of precipitation, the loss of Nb in solid solution by the formation of metastable L21 needles and stable λ, Nb(Fe1–xAlx)2 blocky precipitates in these alloys initially has no major effect on hardening, but after long anneals the coarsening of these precipitates results nevertheless in softening. Stress-strain curves for Nb2Fe73Al25 have been measured at different temperatures and strain rates by [2004Mor2, 2006Mor1]. The rapid formation and coarsening of the λ, Nb(Fe1–xAlx)2 phase above 700˚C is detrimental for the high temperature strength of these alloys [2005Mor]. This limits the use of these alloys to 700–800˚C, and even lower temperatures (< 600˚C) are recommended for longterm applications. [1991Ran] used combustion synthesis to prepare two-phase microstructures consisting of Fe3Al and Nb2Fe for which sufficiently high strength can be retained up to 700˚C. Compression tests on these alloys indicate the possibility of superplasticity around 900˚C. The brittle-to-ductile transition for the two-phase alloys Nb5.1Fe62.2Al32.7 and Nb16.7Fe53.9Al29.4 has been measured by [1996Mac]. [1997Par] studied the effect of Nb addition on the precipitation strengthening and fracture mechanisms in Fe-25Al alloys. [1999Den] has performed calculations on the density of the valence electrons to describe the effect of Nb additions on the grain boundary and bulk bond strength in Fe-25Al. [1998Aud2] investigated the mechanical and corrosion behavior of partially and fully amorphous Al-rich Al-Fe-Nb alloys as an improved light material. Results indicate that fully amorphous alloys exhibit low Young’s moduli, high microhardness and good corrosion behavior. [1993Kai] studied the corrosion kinetics in H2/H2O/H2S atmosphere in the temperature range 700–980˚C. With increasing Nb addition to Fe-3Al (mass%) the corrosion rate reduces with a most pronounced reduction from 30 to 40 mass% Nb. The addition of 10 mass% Al to Nb-70Fe (mass%) leads at 700 and 800˚C to a significant decrease in corrosion rate. [1997Cho] has observed that the addition of Nb to Fe-25Al (at.%) accelerates both the granular and the intergranular corrosion. Mo¨ssbauer spectroscopy studies on NbxFeAl1–x for 0.1 ≤ x ≤ 0.3 indicate that the FeAl and λ phase (Nb(Fe1–xAlx)2) are paramagnetic down to 85 K [1993Mah]. The Debye temperature for the FeAl phase is 112 ± 5˚C. The magnetic behavior of the λ, Nb(Fe1–xAlx)2 phase in the Al-Fe-Nb system has been calculated through the LAPW method by [2002Ima]. Information on the type of property and the used technique or method in these investigations is given in Table 4.
Miscellaneous [1990Car] performed ab initio electronic band calculations to predict the effect of Fe addition on the relative stability between the tetragonal D022 and cubic L12 structure for the NbAl3 phase. Although he assumes in contradiction to [1989Sub] that Fe substitutes for Al in the DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
tetragonal D022 structure, their conclusions that Fe is not an efficient stabilizer of the cubic structure, are in agreement. [1999Mek] used a quasichemical method based on statistico-thermodynamical theory in combination with electronic theory in the pseudopotential approximation to determine the effect of Nb on the ordering in the FeAl phase. In NbxFe0.5Al0.5–x alloys with x up to 0.005, the Nb atoms preferentially occupy the Fe sublattice sites and the normalized critical orderdisorder phase transformation temperature change by addition of Nb, ΔT/TO, varies from 47.35 for x = 0.00125 to 202.17 for x = 0.005. According to [2002Boz], however, the BozzoloFerrante-Smith method based on quantum approximate methods predicts that Nb will preferentially occupy the Al lattice sites in the B2 compound for both NbxFe0.5Al0.5–x and NbxFe0.5–xAl0.5. Several investigations have been focussed on the addition of Nb to alloys with a composition around Fe-25Al. Especially the effect of Nb on the ordered D03 and B2 and the disordered A2 structure has been studied. The temperature change for the D03 Ð B2 transition through addition of Nb has been measured by [1995Ant], [2003Ste], [2005Mor] and [2006Gol] with a maximum of about 100˚C for 1.5–2 at.% Nb. The B2 Ð A2 transition as determined by [2003Ste] and [2005Mor] shows a similar behavior. [2005Gol, 2006Gol] investigated the relaxation phenomena and atom diffusivity in Fe74Al26 with 0.005 to 0.04 at.% C and with and without 0.3 at.% Nb. Nb is supposed to occupy the FeI sites (4b) in the D03-order which gives the L21 structure. From the small change in 59Fe bulk diffusivity through the addition of 0.3 at.% Nb, it is deduced that Nb practically does not influence the vacancy concentration in the as-quenched B2 state. Nevertheless, the segregation of Nb to the grain boundaries results in a decrease of the Fe grain boundary self-diffusion by a factor of 2 to 3 at 1050 K. [1991Sik] describes the melting of Fe-25Al alloys with Nb and other additions by arc melting, air-induction melting, vacuum-induction melting, vacuum-arc remelting and electroslag remelting. The effect of solidification rate on the microstructure of Nb9.1Fe49.3Al41.2 and Nb9.7Fe67.5Al22.8 has been described in respectively [1999Mot] and [2005Mot]. XRD and Mo¨ssbauer studies of [1993Mah] on the FeAl phase and λ phase (Nb(Fe1–xAlx)2) within NbyFeAl1–y alloys with 0.1 ≤ y ≤ 0.3 show that neither phase is pure and stoichiometric. The lattice parameter a of FeAl is constant at 291 pm for all y, which is higher than the observed values for pure FeAl with less than 50 at.% Al. The lattice parameters a and c of λ decrease gradually from 496 to 491 pm, and from 812 to 800 pm as y increases from 0.1 to 0.3, thereby indicating the replacement of Fe by Al atoms. Investigations on the atomic structure, glass forming ability and crystallization behavior of partially or fully amorphous rapidly solidified Al-rich Al-Fe-Nb alloys have been performed for the composition Nb10Fe20Al70 by [1988Tsa], for Nb5Fe8Al87, Nb3Fe13Al84 and Nb10Fe10Al80 by [1997Aud2], for Nb3Fe10Al87 by [1997Aud1, 1998Aud1, 2004Aud]. In [1998Aud2] the mechanical and corrosion properties of (partially) amorphous Nb3Fe10Al87 alloys are discussed. These investigations show that through a proper choice of alloy composition and heat treatment, it is possible to prepare nanocomposites with an amorphous matrix containing metallic nanocrystals. [2001Rod] found that the high-energy ball milling of Nb5Fe5Al90 and Nb3Fe7Al90 also results in a composite microstructure with amorphous and nanocrystalline regions for which the effect of heat treatment on the microstructure is described in [2001Rod, 2003Rod].
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
5
6
8
Al–Fe–Nb
In the review of [2004Mor1] it is mentioned that the λ, Nb(Fe1–xAlx)2 phase has intermediate level of high temperature solubility and low temperature stability in comparison to possible carbides, oxides and nitrides in iron aluminides.
. Table 1 Investigations of the Al-Fe-Nb Phase Relations, Structures and Thermodynamics Reference
Method/Experimental Technique
Temperature/Composition/Phase Range Studied
[1966Ram]
X-ray investigation
1000˚C, 24 alloys in all composition range
[1970Bur]
X-ray and microstructural investigation
800˚C, 153 alloys in all composition range
[1971Dub]
Isothermal calorimetry using aluminothermic reduction reaction
(Nb0.38Fe0.62)100–xAlx with x = 1.3–6.3 (mass%) and (Nb0.68Fe0.32)100–xAlx with x = 1.9–9.5 (mass%)
[1985Tro]
X-ray powder diffraction, hardness
900–1200˚C, Nb0.8Fe2Al0.2 (at.%)
[1986Bla]
X-ray powder diffraction, hardness
800–1200˚C, NbFe2 to Nb0.5Fe2Al0.5 (at.%)
[1988Dim]
Transmission electron microscopy (SAED and CBED), electron probe microanalysis
600–800˚C, Nb2Fe73Al25 (at.%)
[1990Car]
Ab initio total energy and density of states calculation
Nb(Fe1–xAlx)3 with x = 0.167 and 0.334 (at.%)
[1993Mah]
X-ray diffraction, Mo¨ssbauer spectroscopy
830˚C, FeAl1–xNbx with 0.1≤ x ≤0.3 (at.%)
[1995Ant]
Differential scanning calorimetry
60˚C ≤ T ≤ 1030˚C, NbxFe74–xAl26 with 1 ≤ x ≤ 3 (at.%)
[1996Mac]
Optical and transmission electron T ≤ 1400˚C, Nb33.4Fe33.6Al33.0, microscopy, X-ray diffraction at room and Nb5.1Fe62.2Al32.7, Nb16.7Fe53.9Al29.4 (at.%) high temperature
[1999Mek]
Calculation using a quasi-chemical T = 1000–1250˚C, NbxFe0.5Al0.5–x with method combined with electronic theory x ≤ 0.005 (at.%) in the pseudopotential approximation
[1999Mot]
Directional solidification experiments, optical microscopy
Nb9.7Fe67.5Al22.8, Nb9.1Fe49.7Al41.2, Nb8.0Fe47.0Al45.0 (at.%)
[2001Rod]
X-ray diffraction, scanning electron microscopy, transmission electron microscopy, differential scanning calorimetry
T ≤ 600˚C, Nb5Fe5Al90, Nb3Fe7Al90 (at.%)
[2001Sud]
Thermodynamical calculation of enthalpy Al-Fe-Nb liquid of mixing
[2004Aud]
X-ray diffraction, transmission electron microscopy, differential scanning calorimetry
[2004Mor2] Transmission electron microscopy
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
T = 550˚C, Nb3Fe7Al90, Nb3Fe10Al87 (at.%)
T = 900 and 1300˚C, Nb2Fe73Al25 (at.%) Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
. Table 1 (continued) Reference
Method/Experimental Technique
Temperature/Composition/Phase Range Studied
[2005Gol]
Internal friction using a vibrating-reed apparatus and an inverted torsion pendulum, positron annihilation spectroscopy, radiotracer diffusion measurements, transmission electron microscopy
1000˚C ≤ T ≤ 1250˚C, Nb0.3Fe73.7Al26 (at.%)
[2005Mor]
X-ray diffraction, transmission electron microscopy, scanning electron microscopy
as quenched from T = 1200˚C and annealed at T = 500 to 900˚C, Nb2Fe73Al25, Nb5Fe75Al20 (at.%)
[2005Mot]
Directional solidification experiments, T ≤ 1400˚C, Nb9.7Fe67.5Al22.8 (at.%) optical and scanning electron microscopy
[2006Gol]
Anelastic relaxation using a vibratingreed apparatus and an inverted torsion pendulum
[2006Mor1] Transmission electron microscopy, hardness
700˚C ≤ T ≤ 1100˚C, Nb0.3Fe73.7Al26 (at.%)
T ≤ 900˚C, Nb2Fe73Al25 (at.%)
. Table 2 Crystallographic Data of Solid Phases
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
(Al) < 660.452
cF4 Fm 3m Cu
(αδFe) (αFe) < 912 (δFe) 1538 - 1394
cI2 Im 3m W
(γFe) 1394 - 912 (Nb) < 2469
Landolt‐Bo¨rnstein New Series IV/11E1
Lattice Parameters [pm]
Comments/References
a = 404.96
pure Al at 25˚C [Mas2]
a = 286.65
at 25˚C [Mas2]
a = 293.15
[Mas2] Strukturbericht designation: A2
cF4 Fm 3m Cu
a = 364.67
at 915˚C [V-C2, Mas2]
cI2 Im 3m W
a = 330.04
pure Nb at 25˚C [Mas2]
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
7
8
8
Al–Fe–Nb
. Table 2 (continued)
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Fe4Al13 < 1160
mC102 C2/m Fe4Al13
Fe2Al5 < 1169
oC24 Cmcm Fe2Al5
FeAl2 < 1156
aP18 P1 FeAl2
ε, Fe2Al3 1232 - 1102
cI16
α2, FeAl < 1310
cP2 Pm 3m CsCl
Fe3Al < 552
cF16 Fm 3m BiF3
NbAl3 < 1680
tI8 I4/mmm TiAl3
Lattice Parameters [pm]
a = 1549.2±0.2 76.0 at.% Al [1994Gri] b = 807.8 ± 0.2 c = 1247.1 ± 0.1 β = 107.69 ± 0.01˚ 70 to 73 at.% Al [1993Kat] at 71.5 at.% Al [1994Bur]
a = 767.5 b = 640.3 c = 420.3 a = 487.8 b = 646.1 c = 880.0 α = 91.75˚ β = 73.27˚ γ = 96.89˚
66 to 66.9 at.% Al [1993Kat] at 66.9 at.% Al [V-C2]
58 to 65 at.% Al [1993Kat] at 61 at.% Al [V-C2]
a = 598.0
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
Comments/References
a = 289.53 a = 289.66 a = 289.77 a = 290.17 a = 290.9
a = 579.30 a = 578.86
a = 384.1 c = 860.9
24 to 55 at.% Al [1993Kat] at 36.2 at.% Al at 38.3 at.% Al at 40.9 at.% Al at 43.8 at.% Al at 50 at.% Al [1958Tay] Strukturbericht designation: B2 25 to 37 at.% Al [2001Ike] at 23.1 at.% Al at 35.0 at.% Al [1958Tay] Strukturbericht designation: D03 Nb solubility: 1 at.% at 1300˚C [2004Mor2] 2 at.% at 1300˚C [1988Dim] 1.6 at.% at 1150˚C [2003Ste] 0.87 at.% at 1000˚C [2003Ste] 1 at.% at 1000˚C [1988Dim] 0.5 at.% at 700˚C [1988Dim] [V-C2] Strukturbericht designation: D022 5 at.% at 1000˚C [1966Ram]
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
. Table 2 (continued)
Phase/ Temperature Range [˚C] σ, Nb2Al < 1940
Pearson Symbol/ Space Group/ Prototype tP30 P42/mnm σCrFe
Lattice Parameters [pm]
Comments/References 30 to 42 at.% Al [Mas2] at 32 at.% Al
a = 995.2 c = 516.8 a = 989.6 c = 518.7
at 42 at.% Al [1980Jor] Fe solubility: 10 at.% at 1000˚C [1966Ram] 2 at.% at 800˚C [1970Bur]
Nb3Al < 2060
cP8 Pm 3n Cr3Si
μ, Nb19(Fe1–xAlx)21 Nb19Fe21
hR39 R 3m
< 1530
W6Fe7
μ’, Nb2FeAl
-
λ, Nb(Fe1–xAlx)2 NbFe2 < 1630
hP12 P63mmc MgZn2
τ Nb73–xFe10–yAl17+x+y -
Landolt‐Bo¨rnstein New Series IV/11E1
a = 518.6
18.6 to 25 at.% Al [Mas2]
0 ≤ x ≤0.4 [1966Ram] 48 to 52 at.% Nb (1100 to 1500˚C) [1993Bej1] a = 492.8 c = 268.3
for Nb6Fe7 [V-C2] Al solubility: 20 at.% at 1000˚C [1966Ram] μ type related crystal structure [1966Ram]
-
0 ≤x ≤ 0.75 [1966Ram] [1987Rag]
a = 482.6 c = 787.2 a = 483.2 c = 789.1 a = 483.2 c = 788.3 a = 482.8 c = 787.1 a = 483.8 c = 787.7 a = 484.6 c = 789.2 a = 496.7 c = 807.8
Nb0.9Fe2Al0.1 [1986Bla] Nb0.8Fe2Al0.2 [1985Tro] Nb0.7Fe2Al0.3 [1986Bla] Nb0.6Fe2Al0.4 [1986Bla] Nb0.5Fe2Al0.5 [1986Bla] Nb33.4Fe33.6Al33.0 [1996Mac] 0 ≤ x ≤ 5, 0 ≤ y ≤ 5 approximate concentration deduced from isothermal section at 1000˚C [1999Mot]
-
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
9
10
8
Al–Fe–Nb
. Table 3 Thermodynamic Data of Reaction or Transformation Reaction or Transformation
T [˚C]
Quantity, per mole of atoms [kJ, mol, K]
Comments
(100–x)Nb0.38Fe0.62(L) + xAl(L) Ð (Nb0.38Fe0.62)(100–x) Alx(L)
ΔsH = 105 ± 13 kJ·mol–1
x = 1.3–6.3 (mass%) Heat of solution by isothermal calorimetry using aluminothermic reaction [1971Dub]
(100–x)Nb0.68Fe0.32(L) + xAl(L) Ð (Nb0.68Fe0.32)(100–x) Alx(L)
ΔsH = 100 ± 13 kJ·mol–1
x = 1.9–9.5 (mass%) Heat of solution by isothermal calorimetry using aluminothermic reaction [1971Dub]
(100–x)NbyFe1–y(L) + xAl(L) Ð (NbyFe1–y)(100–x) Alx(L)
ΔmH = –(5–10) kJ·mol–1 ΔmH = –(20–25) kJ·mol–1 ΔmH = –(5–10) kJ·mol–1 ΔmH = –(15–20) kJ·mol–1
x = 0 at.%, y = 0.5 x = 50 at.%, y = 0 x = 50 at.%, y = 1 x = 33 at.%, y = 0.5 Calculated enthalpy of mixing [2001Sud]
. Table 4 Investigations of the Al-Fe-Nb Materials Properties Reference
Method / Experimental Technique
Type of Property
[1986Bla]
PMT-3 metallographic microscope with 100 and 200 gf load
Microhardness
[1991Ran]
Compression tests
Strength, superplastic behavior
[1993Kai]
Corrosion tests in H2/H2O/H2S atmospheres
Corrosion behavior
[1993Mah]
Mo¨ssbauer spectroscopy
Magnetic behavior
[1996Mac]
Vickers hardness, Compression and 4-point bending test
Vickers hardness, brittle-to-ductile transition temperature, stress-strain curve
[1997Cho]
Potentiostatic measurements
Corrosion behavior
[1997Par]
Yield strength measurements, Vickers hardness, charpy impact test
Strength, fracture behavior
[1998Aud2] Microhardness, nanoindentation, potentiodynamic polarization in a chloride containing solution
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
Mechanical and corrosion behavior
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
. Table 4 (continued) Reference
Method / Experimental Technique
Type of Property
[1999Den]
Positron lifetime measurements and calculations of density of valence electrons and grain boundary cohesion
Fracture behavior
[2002Ima]
Ab initio calculations (LAPW)
Magnetic properties
[2004Mor2] Compression tests
Strength
[2005Mor]
Strength
Microscopical investigation by transmission electron microscopy and X-ray diffractions
[2006Mor2] Vickers microhardness testing with 200 g load Hardness [2006Mor1] Vickers microhardness testing with 100 g load, Stress-strain curve, yield stress, compression testing hardness
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
11
12
8
Al–Fe–Nb
. Fig. 1 Al-Fe-Nb. The Fe-Nb phase diagram
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
. Fig. 2 Al-Fe-Nb. Tentative liquidus surface in the Fe corner
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
13
14
8
Al–Fe–Nb
. Fig. 3 Al-Fe-Nb. Isothermal section at 1000˚C
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb
8
. Fig. 4 Al-Fe-Nb. Isothermal section at 800˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
15
16
8
Al–Fe–Nb
References [1958Tay] [1962Min]
[1966Lun] [1966Ram] [1970Bur]
[1971Dub]
[1980Jor] [1981Ell] [1982Kub] [1985Tro] [1986Bla] [1987Rag]
[1988Dim]
[1988Tsa] [1989Sub]
[1990Car] [1990Kum] [1991Bej]
[1991Ran]
[1991Sik] [1992Gam]
Taylor, A., Jones, R.M., “Constitution and Magnetic Properties of Iron Rich Iron-Aluminium Alloys”, J. Phys. Chem. Solids, 6, 16–37 (1958) (Crys. Structure, Experimental, 49) Mints, R.S., Samsonova, N.N., Malkov, Y.S., “The Effects of Elements of Group V in the Periodic System (V, Nb, Ta) on the Properties of Fe3Al” (in Russian), Dokl. Akad. Nauk SSSR, 144(6), 1324–1327 (1962) (Experimental, Electr. Prop., Mechan. Prop., 6) cited from abstract Lundin, C.E., Yamamoto, A.S., “The Equilibrium Phase Diagram, Niobium (Columbium)Aluminum”, Trans. Met. Soc. AIME, 236, 863–872 (1966) (Phase Diagram, Experimental, 20) Raman, A., “X-ray Investigations in Several T-T5-Al Systems” (in German), Z. Metallkd., 57(7), 535–540 (1966) (Phase Diagram, Phase Relations, Experimental, #, 5) Burnashova, V.V., Ryabov, V.R., Markiv, V.Y., “Investigation of the Nb-Fe-Al and Nb-Co-Al Systems”, Dopov. Akad. Nauk Ukr. RSR, Ser. A: Fiz.-Mat. Tekh. Nauki, A8, 747–750 (1970) (Phase Diagram, Experimental, Phase Relations, #, 11) Dubrovin, A.S., Gorelkin, O.S., Demidov, Yu.Ya., Chirkov, N.A., Kostylev, L.S., Kolesnikova, O.D., “Calorimetric Investigation of Heat Solution of Silicon and Aluminium in Aluminium Thermal Alloys” (in Russian), Metallotherm. Process. Khim. Met. Mater. 1971, 121–130 (1971) (Thermodyn., Experimental, 11) Jorda, J.L., Fluekiger, R., Mueller, J., “A New Metallurgical Investigation on the Niobium-Aluminium System”, J. Less-Common Met., 75, 227–239 (1980) (Phase Diagram, Experimental, #, 20) Elliott R.P., Shunk, F.A., “The Al-Nb System”, Bull. Alloy Phase Diagrams, 2, 75–81 (1981) (Phase Diagram, Crys. Structure, Review, 31) Kubaschewski, O., “Al-Fe” in “Iron Binary Phase Diagrams”, Springer Verlag, Berlin 5–9 (1982) (Phase Diagram, Review, 26) Trojko, R., Blazina, Z., “Metal-Metalloid Exchange in some Friauf-Laves Phases Containing Two Transition Metals”, J. Less-Common Met., 106, 293–300 (1985) (Crys. Structure, Experimental, 13) Blazina, Z., Trojko, R., “Structural Investigations of the Nb1–xSixT2 and Nb1–xAlxT2 (T = Cr, Mn, Fe, Co, Ni) Systems”, J. Less-Common Met., 119, 297–305 (1986) (Crys. Structure, Experimental, 6) Raghavan, V., “Section I. The Al-Fe-Nb (Aluminum-Iron-Niobium) System”, Phase Diagrams of Ternary Iron Alloys. Part 1, Ind. Inst. Techn. Delhi, 1, 3–8 (1987) (Crys. Structure, Phase Diagram, Phase Relations, Review, 8) Dimiduk, D.M., Mendiratta, M.G., Banerjee, D., Lipsitt, H.A., “A Structural Study of Ordered Precipitates in an Ordered Matrix within the Fe-Al-Nb System”, Acta Metall., 36(11), 2947–2958 (1988) (Phase Relations, Morphology, Experimental, 17) Tsai, A.-P., Inoue, A., Masumoto, T., “A New Icosahedral Al-Fe-Ta Alloy Prepared by Rapid Solidification”, Jpn. J. Appl. Phys., 27(1), L5-L8 (1988) (Experimental, Morphology, 18) Subramanian, P.R., Simmons, J.P., Mendiratta, M.G., Dimiduk, D.M., “Effect of Solutes on Phase Stability in Al3Nb”, Mater. Res. Soc. Symp. Proc., 133(3), 51–56 (1989) (Phase Diagram, Experimental, Mechan. Prop., 12) Carlsson, A.E., Meschter, P.J., “Relative Stabilities of L12 and DO22 Structures in Ternary Mal3-Base Aluminides”, J. Mater. Res., 5(12), 2813–2818 (1990) (Crys. Structure, Thermodyn., Experimental, 15) Kumar, K.S., “Ternary Intermetallics in Aluminium-Refractory Metal-X Systems (X = V, Cr, Mn, Fe, Co, Ni, Cu, Zn)”, Int. Mater. Rev., 35(6), 293–327 (1990) (Crys. Structure, Phase Diagram, Review, 158) Bejarano, Z.J.M. Gama, S., Ribeiro, C.A., Effenberg, G., Santos, G., “On the Existence of the Fe2Nb3 Phase in the Fe-Nb System”, Z. Metallkd., 82, 615–620 (1991) (Phase Diagram, Phase Relations, Experimental, 7) Ranganath, S., Dutta, A., Subrahmanyam, J., “On the flow Behaviour of Combustion Synthesized FeAl-Nb System”, Scr. Metall. Mater., 25(7), 1593–1596 (1991) (Morphology, Experimental, Mechan. Prop., 6) (cited from abstract) Sikka, V.K., “Production of Fe3Al-Based Intermetallic Alloys”, Mater. Res. Soc. Symp. Proc.: High-Temp. Ordered Intermetallic Alloys IV, 213, 907–912 (1991) (Experimental, 2) Gama, S., “Aluminium - Iron - Niobium”, MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.18061.1.20, (1992) (Crys. Structure, Phase Diagram, Assessment, 10)
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Fe–Nb [1993Bej1] [1993Bej2] [1993Kai] [1993Kat]
[1993Mah]
[1994Bur]
[1994Gri]
[1995Ant] [1996Mac] [1997Aud1] [1997Aud2] [1997Cho]
[1997Par]
[1998Aud1]
[1998Aud2]
[1999Den]
[1999Mek]
[1999Mot]
[2001Ike]
[2001Rod] [2001Sud]
8
Bejarano, Z.J.M., Gama, S., Ribeiro, C.A., Effenberg, G., “The Iron-Niobium Phase Diagram”, Z. Metallkd., 84, 160–164 (1993) (Experimental, Phase Diagram, #, 6) Bejarano, Z.J.M, PhD Thesis, State Uni. Campinas, Brazil (1993) as quoted in [1999Mot] Kai, W., Douglass, D.I., “The Corrosion Behaviour of Fe-Nb-Al alloys in H2/H2O/H2S Atmospheres”, Oxidation of Metals, 39(5-6), 317–352 (1993) (Electrochem., Experimental, 12) (cited from abstract) Kattner, U.R., Burton, B.P., “Al-Fe (Aluminum-Iron)” in “Phase Diagrams of Binary Iron Alloys”, Okamoto, H. (Ed), ASM International, Materials Park, OH 44073–0002, 12–28 (1993) (Crys. Structure, Phase Diagram, Thermodyn., Review, Electr. Prop., Magn. Prop., 99) Mahmood, S.H., Awawdeh, M.A., Saleh, A.S., “Structural and Mossbauer Studies of the Alloy System FeAl1–xNbx”, J. Appl. Phys., 73(10), 5663–5665, part 2A (1993) (Phase Relations, Experimental, Magn. Prop., 12) Burkhardt, U., Grin, J., Ellner, M., Peters, K., “Structure Refinement of the Iron-Aluminum Phase with the Approximate Composition Fe2Al5”, Acta Crystallogr., Sect. B: Struct. Crystallogr. Crys. Chem., 50, 313–316 (1994) (Crys. Structure, Experimental, 9) Grin, J., Burkhardt, U., Ellner, M., Peters, K., “Refinement of the Fe4Al13 Structure and its Relationship to Quasihomological Homeotypical Structures”, Z. Kristallogr., 209, 479–487 (1994) (Crys. Structure, Experimental, 39) Anthony, L., Fultz, B., “Effect of Early Transition Metal Solutes on the D03 - B2 Critical Temperature of Fe3Al”, Acta Metall. Mater., 43(10), 3885–3891 (1995) (Phase Relations, Experimental, 35) Machon, L., Sauthoff, G., “Deformation Behaviour of Al-Containing C14 Laves Phase Alloys”, Intermetallics, 4, 469–481 (1996) (Phase Relations, Experimental, 41) Audebert, F, Sirkin, H., Escorial, A.G., “Approach to the Atomic Structure of Amorphous Al-Fe-Nb”, Philos. Mag. B, 76(4), 483–487 (1997) (Electronic Structure, Experimental, 18) (cited from abstract) Audebert, F, Sirkin, H., Escorial, A.G., “Aluminum-base Al-Fe-Nb Amorphous and Nanostructured Alloys”, Scr. Mater., 36(4), 405–410 (1997) (Morphology, Experimental, 19) Choe, H.-C., Choi, D.-C., “Effects of Cr, Mo, Nb and B on the Intergranular Corrosion Behaviour of Fe-25 at.% Al Intermetallic Compounds”, J. Korean Inst. Met. Mater., 35(4), 468–476 (1997) (Electrochem., Experimental, 16) (cited from abstract) Park, K.-I., Joo, S.-M., Choi, D.-C., “Effects of Cr, Mo, Nb and B Additions on the Microstructure and Mechanical Properties in Fe-25 at.% Al Alloy”, J. Korean Inst. Met. Mater., 35(3), 305–311 (1997) (Morphology, Experimental, Mechan. Prop., 17) (cited from abstract) Audebert, F., Sirkin, H., Escorial, A.G., “Study of the Crystallisation Process of the Al-Fe-Nb Amorphous Alloys”, Proceedings of the Fifth International Workshop on Non-Crystalline Solids. NonCrystalline and Nanoscale Materials. World Scientific. 1998, Singapore, Singapore, 367–372 (1998) (Morphology, Experimental, 19) (cited from abstract) Audebert, F., Vazquez, S., Gutierrez, A., Vergara, I., Alvarez, G., Garcia Escorial, A., Sirkin, H., “Mechanical and Corrosion Behaviour of Al-Fe-Nb Amorphous Alloys”, Mechanically Alloyed, Metastable and Nanocrystalline Materials, part 2, Mater. Sci. Forum, 269-272, 837–842 (1998) (Electrochemistry, Experimental, Mechan. Prop., 17) (cited from abstract) Deng, W., Zhong, X.P., Huang, Y.Y., Xiong, L.Y., Wang, S.H., Guo, J.T., Long, Q.W., “Effects of Nb and Si on Densities of Valence Electrons in Bulk and Defects of Fe3Al Alloys”, Sci. China, Ser. A, 42(1), 87–92 (1999) (Electronic Structure, Experimental, 15) (cited from abstract) Mekhrabov, A.O., Akdeniz, M.V., “Effect of Ternary Alloying Elements Addition on Atomic Ordering Characteristics of Fe-Al Intermetallics”, Acta Mater., 47(7), 2067–2075 (1999) (Thermodyn., Calculation, Theory, 63) Mota, M.A., Coelho, A.A., Bejarano, J.M.Z., Gama, S., Caram, R., “Directional Growth and Characterization of Fe-Al-Nb Eutectic Alloys”, J. Cryst. Growth, 198(part 1), 850–855 (1999) (Phase Relations, Experimental, 19) Ikeda, O., Ohnuma, I., Kainuma, R., Ishida, K., “Phase Equilibria and Stability of Ordered BCC Phases in the Fe-rich Portion of the Fe-Al System”, Intermetallics, 9, 755–761 (2001) (Phase Diagram, Experimental, Mechan. Prop., 18) Rodriguez, C.A.D., Botta, F.W.J., “High-Energy Ball Milling of Al-Based Alloys”, Key Eng. Mater., 189191, 573–578 (2001) (Crys. Structure, Experimental, 10) Sudavtsova, V.S., Vovkotrub, N.E., Kudin, V.G., “Thermodynamic Properties of the Fe-Nb(Ta,W), Fe-Nb(Ta,W)-Al Alloys” (in Russian), Metally, (2), 18–20 (2001) (Thermodyn., Experimental, 7)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
17
18
8 [2002Boz] [2002Ima]
[2003Rod]
[2003Ste]
[2004Aud]
[2004Mor1]
[2004Mor2] [2005Gol]
[2005Mor] [2005Mot]
[2006Gol]
[2006Mor1]
[2006Mor2] [2006MSIT]
[Mas2] [V-C2]
Al–Fe–Nb Bozzolo, G.H., Noebe, R.D., Amador, C., “Site Occupancy of Ternary Additions to B2 Alloys”, Intermetallics, 10, 149–159 (2002) (Crys. Structure, Review, 27) Imaizumi, M., Las, B., Bejarano, J.M.Z., Gama, S., Coelho, A.A., Mota, M.A., Caram, R., “The Magnetic Properties of Fe-Al-Nb Intermetallic Compounds”, Intermag Europe 2002 Digest of Technical Papers, 2002 IEEE international Magnetics Conference, (Cat.No.02CH37323), Piscataway, NJ, USA, AR12 (2002) (Calculations, Magn. Prop., 5) (cited from abstract) Rodriguez C.A.D., Yavari, A.R., Kiminami, C.S, Botta F.W.J., “Milling and Hot Consolidation of Al-FeNb Alloy”, Mater. Sci. Forum, 415-418, 287–292 (2003) (Morphology, Experimental, 18) (cited from abstract) Stein, F., Schneider, A., Frommeyer, G., “Flow Stress Anomaly and Order-disorder Transition in Fe3Albased Fe-Al-Ti-X Alloys with X = V, Cr, Nb, or Mo”, Intermetallics, 11, 71–82 (2003) (Phase Relations, Experimental, 53) Audebert, F., Mendive, C., Vidal, A., “Structure and Mechanical Behaviour of Al-Fe-X and Al-Ni-X Rapidly Solidified Alloys”, Mater. Sci. Eng. A, 375-377, 1196–1200 (2004) (Electronic Structure, Experimental, 22) Morris, D.G., Munoz-Morris, M.A., Chao, J., “Development of High Strength, High Ductility and High Creep Resistant Iron Aluminide”, Intermetallics, 12(7-9), 821–826 (2004) (Interface Phenomena, Morphology, Phase Relations, Review, Mechan. Prop., 52) Morris, D.G., Munoz-Morris, M.A., Baudin, C., “The High-Temperature Strength of Some Fe3Al Alloys”, Acta Mater., 52(9), 2827–2836 (2004) (Morphology, Experimental, Mechan. Prop., 44) Golovin, I.S., Divinski, S.V., Cizek, J., Prochazka, I., Stein, F., “Study of Atom Diffusivity and Related Relaxation Phenomena in Fe3Al-(Ti,Nb)-C Alloys”, Acta Mater., 53(9), 2581–2594 (2005) (Thermodyn., Transport Phenomena, Experimental, 40) Morris, D.G., Requejo, L.M., Munoz-Morris, M.A., “A Study of Precipitation in D03 Ordered Fe-Al-Nb Alloy”, Intermetallics, 13(8), 862–871 (2005) (Morphology, Phase Relations, Experimental, 29) Mota, M.A., Coelho, A.A., Bejarano, J.M.Z., Gama, S., Caram, R., “Fe-Al-Nb Phase Diagram Investigation and Directional Growth of the (Fe,Al)2Nb-(Fe,Al,Nb)ss Eutectic System”, J. Alloys Compd., 399(1-2), 196–201 (2005) (Phase Relations, Experimental, 18) Golovin, I.S., Strahl, A., Neuhaeuser, H., “Anelastic Relaxation and Structure of Ternary Fe-Al-Me Alloys with Me = Co, Cr, Ge, Mn, Nb, Si, Ta, Ti, Zr”, Int. J. Mater. Res. (Z. Metallkd.), 97(8), 1078–1092 (2006) (Crys. Structure, Morphology, Phase Relations, Thermodyn., Experimental, Mechan. Prop., 79) Morris, D.G., Munoz-Morris, M.A., Requejo, L.M., Baudin, C., “Strengthening at High Temperatures by Precipitates in Fe-Al-Nb Alloys”, Intermetallics, 14, 1204–1207 (2006) (Morphology, Phase Relations, Experimental, Mechan. Prop., 24) Morris, D.G., Requejo, L.M., Munoz-Morris, M.A., “Age Hardening in some Fe-Al-Nb Alloys”, Scr. Mater., 54(3), 393–397 (2006) (Morphology, Phase Relations, Experimental, Mechan. Prop., 16) “Al-Fe (Aluminum-Iron)”, Diagrams as Published, in MSIT Workplace, Effenberg, G. (Ed.), Materials Science International Services, GmbH, Stuttgart; Document ID: 30.10236.1.20, (2006) (Crys. Structure, Phase Diagram, Phase Relations, #, 11) Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
DOI: 10.1007/978-3-540-88053-0_8 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
Aluminium – Molybdenum – Nickel Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Kostyantyn Korniyenko, Vasyl Kublii
Introduction Experimental investigations of the phase equilibria in the Al-Mo-Ni system were started by [1925Pfa] and [1933Roe] and, as summarized in [1976Mon], concerned the Ni-rich corner as well as the influence of additions of Mo and Ni on the Al solid solution, respectively. The investigations of the partial Ni-NiAl-Mo system were further developed by [1959Gua2, 1960Bag, 1965Ram, 1976Jac, 1977Aig, 1977Pea, 1978Gul, 1983Nas, 1983Wak, 1984Kov1, 1984Kov2, 1984Mir, 1985Nas, 1986Mas1, 1986Mas2, 1988Mas, 1989Mas, 1989Hon1, 1989Hon2, 1991Mis]. Results of phase equilibria studies for the Al-rich corner are presented by a series of isothermal sections [2002Gru]. The complete ternary system has been investigated experimentally at 600˚C [1971Pry], 800˚C [1969Mar] and 950˚C [1969Vir]. For preparation of the alloys most of the authors used arc melting, while [1971Pry] and [2002Gru] applied levitation induction melting, and [1984Mir] obtained specimens by both conventional arc-casting and powder metallurgy techniques. The traditional methods of investigations were X-ray diffraction (XRD), metallography, differential thermal analysis (DTA), electron microprobe analysis (EMPA). Some authors used scanning electron microscopy (SEM) [1989Hon1, 1989Hon2, 1991Mis, 2002Gru], transmission electron microscopy (TEM) [2002Gru], as well as energy-dispersive X-ray spectroscopy (EDXS) [1991Mis]. Calculations of phase equilibria were carried out by [1974Kau, 1999Kau] and [1999Lu]. A critical review of literature data on phase equilibria in the Al-Mo-Ni system was presented in the assessment of [1993Kub]. Further experimental studies are necessary in order to construct the liquidus surface and the reaction scheme of the complete ternary system as well as isothermal sections in the whole range of compositions.
Binary Systems The Al-Mo, Al-Ni and Mo-Ni systems are accepted from [2005Sch], [2004Sal] and [Mas2], respectively.
Solid Phases Crystallographic data on the known unary, binary and ternary phases are listed in Table 1. [1959Gua2] reported the existence of a ternary phase ψ of composition Mo7,5Ni58,0Al34,5 at Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
1
2
9
Al–Mo–Ni
1175˚C, but did not determine its crystal structure. However, the data of [1960Bag, 1969Mar, 1971Pry, 1983Nas] and [1984Mir] did not confirm its existence. A phase of similar composition was easily obtained by [1969Vir] in the alloys (at.%) Mo50Ni25Al25, Mo43Ni31Al26 and Mo9Ni53Al38, the latter being fairly close to the composition of the reported ψ phase [1959Gua2]. Thus, [1969Vir] concluded that the ψ phase in fact did not belong to the AlMo-Ni system, but was easily stabilized by small amounts of impurities (low purity 99.8 mass% nickel was used for preparation of the specimens!). The ψ phase was indexed as a MgZn2 type Laves phase (a = 474, c = 770 pm). Two ternary compounds have been identified in the Al-rich range of compositions, namely, τ1, Mo(NixAl1–x)3 [1969Mar, 1969Vir, 1971Pry] and τ2. The composition of τ2 was determined by [1969Mar] and [1971Pry] as Mo5Ni18Al77, but [2002Gru] corrected it and determined crystal system and lattice parameters (Table 1). According to the findings of [1969Mar] at 800˚C, [1971Pry] at 600˚C and [1965Ram, 1969Vir] at 950˚C, the τ1 phase is likely to exhibit a homogeneity range strongly dependent on temperature. The compound Mo(Al2,75Ni0,25), observed in the aluminothermic preparation of Al-Mo-Ni alloys from Mo- and Ni-oxides, is likely to be isotypic with the TiAl3 type, despite the fact that the c-axis corresponds to a twofold superstructure [1969Rec]. [1984Och1, 1984Och2, 1985Mis, 1988Mas, 1989Hon1, 1989Hon2] investigated the influence of the addition of a third element on the lattice parameter change of binary Ni solid solutions. The temperature dependence of the solid solubility is reflected in the isothermal sections (see below) and additional information on the γ/γ´ boundary may be obtained from [1989Gai] and [1989Hon1]. A model based on X-ray measurements to show the effect of Mo on the γ´ structure has been suggested by [1977Aig].
Quasibinary Systems On the basis of X-ray, DTA as well as optical microscopy data [1986Mas2] plotted the phase diagram of the partial quasibinary NiAl-Mo system. The temperature of the LÐβ+α equilibrium is equal to 1600±7˚C; the maximum solubility of molybdenum in the β phase is less than 4 at.%. The eutectic point is placed at 10 at.% Mo, and its co-ordinates were later confirmed by [1991Sas]. Part of the quasibinary section in the range of compositions 0 to 20 at.% Mo is presented in Fig. 1, with small changes according to the melting temperature of the β phase at 1651˚C [2004Sal], whereas 1638˚C was accepted by [1986Mas2]. Similar compositions of the eutectic point were reported earlier by [1970Cli] (9 at.% Mo) and [1971Pry] (10 at.% Mo), but considerably lower eutectic temperatures were presented (1427 and 1290˚C, respectively). According to the conclusion of [1993Kub], in view of the high melting temperature of the β phase and the reaction temperature of U1 (1340˚C), the higher quasibinary eutectic temperature (1600˚C) is recommended. The vertical section Mo-Ni3Al, according to the data of [1971Pry], demonstrates a peritectoid reaction β+γÐγ´+α, which is in contradictions to the observation of a eutectic solidification behavior in this area by [1976Spr] and [1983Nas].
Invariant Equilibria The reaction scheme of the partial Mo-NiAl-Ni system is presented in Fig. 2. One invariant three-phase equilibrium as well as six invariant four-phase reactions have hitherto been DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
observed in the system. [1977Pea] reported the equilibrium LÐα+β+γ at 1300˚C, but later it was established by [1977Aig, 1983Nas] and [1983Wak] that instead of the β phase the γ´ phase takes part in the eutectic reaction LÐα+γ+γ´, and the various authors merely agree on the temperature of this reaction at 1300˚C [1977Pea, 1983Wak, 1988Mas]. The reaction temperatures in Fig. 2 were measured and selected by [1986Mas1, 1986Mas2] and [1988Mas]. Table 2 presents the compositions of phases taking part in the invariant equilibria, estimated on the basis of isothermal sections as well as on the data calculated by [1987Sve] and experimentally determined by [1986Mas1] and [1986Mas2].
Liquidus Surface Liquidus surface projection of the Ni-rich region (the Ni-NiAl-Mo partial system) is presented in Fig. 3. It consists of five fields of primary crystallization corresponding to the α, β, γ, γ´ and δ phases. It has been constructed on the basis of constitution of the accepted binary phase diagrams and critically assessed experimental data of different authors. So, the position of the U2E monovariant curve is established using experimental data of [1977Pea, 1984Kov1] and [1984Kov2] on directionally solidified α+γ eutectic superalloys containing 8.58Al-27.22Mo (at.%) up to 18.66Al-15.50Mo (at.%) and 14.38Al-20.03Mo (at.%), as well as data for two alloys, crystallized by [1987Sve] using the Bridgeman method. The position of the U2 invariant point was accepted on the basis of data by [1977Pea] (Table 2), because data by [1987Sve] do not agree with the estimated compositions of the α, δ and γ phases participating in the equilibrium LU2+δÐα+γ at 1310˚C. [1974Tho, 1976Nes, 1976Hen] and [1976Spr] discovered by directional solidification studies the existence of eutectic reactions LÐα+γ´, LÐα+γ and LÐδ+γ. The Ni-NiAl-Mo liquidus surface projection was proposed by [1986Mas2] based on a rather schematic projection given by [1983Nas], but the constitution of the Al-Ni binary as used by [1983Nas] contradicts the assessment of [2004Sal]. A mathematical model was used to construct the isotherms at 1360 and 1340˚C, as well as the monovariant curves p2U2 and U2E [1987Sve, 1989Gai]. Results of thermodynamic calculations of the liquidus surface, carried out by [1999Lu] and based on the experimental data of [1987Sve], were also used in our assessment, except the position of U2, which is placed by [1999Lu] at a smaller Mo content. In Fig. 3 isotherms illustrating the shape of the surface, are added, in particular, the isotherms at 1415, 1425 and 1445˚C, using the experimental data of [1978Gul].
Isothermal Sections Partial isothermal section at 1260˚C is presented in Fig. 4 according to the data of [1984Mir]. Isothermal sections at 1200˚C constructed from the experimental results by [1983Nas] and [1988Mas] are in good agreement with each other and with the calculation performed by [1974Kau], see Fig. 5. The character of phase equilibria in the Ni-rich corner is similar to the character of the assessed equilibria, but the solubility of Mo in the γ´ phase is much smaller than experimental data, and also the position of the γ´+γ two-phase region is different. Phase equilibria at 1100˚C [1988Mas] and 1000˚C [2002Gru] are shown in Figs. 6 and 7, respectively. Figure 8 presents a combination of data at close temperatures: for 1050˚C in the Al-rich range by [2002Gru] and for 1038˚C in the Al-poor range [1984Mir]. Phase equilibria at 927˚C [1984Mir] for Al-poor range and at 950˚C [2002Gru] for Al-rich corner are merged Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
3
4
9
Al–Mo–Ni
in Fig. 9. Partial isothermal sections at 880 (Fig. 10) and 700˚C (Fig. 11) are accepted from [1988Mas]. In the assessed isothermal sections some minor modifications have been made taking into account the newly determined position of the γ/γ´ boundary according to SEM and DTA data by various groups (see “Solid Phases”) and according to the constitution of the boundary systems. In particular, Fig. 11 reflects the participation of the later determined Ni5Al3 phase in the equilibria at 700˚C. [1989Hon1, 1989Hon2] and [1991Mis] confirmed that the extent of the γ(Ni) solid solution area increases with rising temperature. The position of the nickel-rich boundary of the γ´ phase at 1200˚C, calculated by [1991Eno] using the cluster variation method, CVM (which utilizes the tetrahedron approximation and the phenomenological Lennard-Jones pair interaction potential), practically coincides with the data of [1983Nas].
Temperature – Composition Sections Figure 12 shows the partial isopleth at 14 at.% Al for a Ni content changing from 58 to 86 at.% according to the data of [1989Mas]. This isopleth crosses two volumes of primary crystallization, corresponding to the α and γ phases, and four planes of invariant four-phase equilibria, in one of which (at ≈ 1300˚C) the liquid phase takes part, and the others are with participation of only the solid phases (at ≈ 1130, ≈ 890 and ≈ 730˚C). The partial isopleth at 65 at.% Ni with Mo content changing from 15 to 35 at.%, as constructed by [1983Wak], and the isopleths Mo60Al40 - Ni, Mo45Al55 - Ni constructed by [1986Mas2] do not comply with the assessed liquidus surface.
Thermodynamics No experimental thermodynamic data concerning the Al-Mo-Ni system are published in literature. [1974Kau] calculated the isothermal sections at 1727, 1527 and 1200˚C using symmetrical functions for the excess free energies of mixing. There is a substantial disagreement between the calculated and the experimental data; moreover constitution of the calculated binaries Al-Ni, Al-Mo and Mo-Ni contradict the phase diagrams accepted in this assessment. [1999Kau] and [1999Lu] assessed the experimental phase equilibria data in order to evaluate the thermodynamic parameters of the ternary system by means of the CALPHAD method. A substitutional-solution model is used to describe liquid, face-centered cubic (fcc) and body-centered cubic (bcc) phases, while a sublattice model is used to describe the intermetallic phases. Two sets of thermodynamic descriptions have been obtained, and comparison has been made between them. There is satisfactory agreement between the calculations and experimental data. But phase diagrams of the boundary systems Al-Ni, Mo-Ni and Al-Mo, accepted by [1999Kau] and [1999Lu], disagree to some extent with the phase diagrams accepted in this assessment. [2000Bor] presented a general survey of the diffusion-controlled transformations (DICTRA) software as an engineering tool for diffusion simulations in multicomponent alloys. The model of coarsening of the γ´ phase particles in ternary Al-Mo-Ni alloys was used. In the calculation, the alloy composition was adjusted in
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
order to have the same fraction of the γ´ phase as experimentally observed. This gave a small difference in composition compared with the experimental data.
Notes on Materials Properties and Applications The Al-Ni alloys with the addition of a refractory metal element (in particular, molybdenum) are interesting as materials for production of in situ composites of eutectic superalloys that can serve, in particular, as materials for specific hot section components of turbine engines, primarily blades or buckets and vanes as well as nozzles [1976Jac]. In spite of very complicated alloys compositions, commercial superalloys generally consist mainly of two phases, namely, γ and γ´. The β phase has potential applications such as hot sections of gas turbine engines for aircraft propulsion systems, coats under thermal barrier coating, electronic metallization compounds in advanced semiconductors [1998Mur] as well as surface catalysts [1971Nal, 1998Mur]. The influence of molybdenum additions on the structure and hardness of the γ´ phase based alloys has been studied by [1959Gua1], and three general effects have been observed, namely, solid-solution hardening, strain aging, and defect hardening arising from deviations from stoichiometry. A method for the determination of site preference of substitutional elements in intermetallic compounds was proposed by [2001Ter], and it was demonstrated that in the γ´ based alloys molybdenum substitutes preferentially for aluminium. The microstructure and chemical characteristics of the nanocrystalline β phase are studied by [2002Alb]. It was established that the addition of molybdenum tends to slightly refine the grain size of the β phase based alloy. The specimens with 2, 4 or 6 at.% Mo are polycrystalline containing, at the same time, the β phase, Ni, Al and Mo. The cast alloy NiAl-9Mo (at.%), prepared by [2002Guo], exhibited typical deformation characteristics shown in conventionally superplastic materials, and possessed finely grained structure. Properties of the directionally solidified eutectic superalloys were investigated by [1973Wal, 1974Tho, 1976Jac, 1976Nes, 1976Spr, 1981Sch, 1984Sch, 1985Nas, 1986Hor, 1986Kau] and [1987Sve]. It is shown that composites formed by directional eutectic solidification combined with a reinforcing α phase in the form of fibers have a considerable advantage over conventional superalloys [1973Wal, 1974Tho, 1976Jac, 1976Nes, 1976Spr]. Since the microstructure derives directly from the melt, the composites are extremely stable at elevated temperatures. In addition improved oxidation and creep resistances have been observed [1981Sch, 1985Nas]. The characteristic microstructure of the alloys consists of γ/γ´ matrix reinforced with faceted αMo fibres, which are primarily square in cross section and with the following orientation relationship: [001]γ´// [001]α, (010)γ//(010)γ´//(110)α, (100)γ´//(110) [1981Sch, 1984Sch, 1986Hor, 1986Kau, 1987Sve]. Precipitation in Ni-rich Al-Mo-Ni alloys has been investigated in the temperature range 600 to 1100˚C by transmission electron microscopy, selected-area electron diffraction and hardness measurements [1987San]. Various stable and metastable phases (α, γ´ and δ MoNi, MoNi2 (MoPt2 type), MoNi3 (TiAl3 type), MoNi4, MoNi8 and SRO) have been observed and the ranges of alloy composition and aging temperature for which each phase is formed have been determined and their strengthening influence on the mechanical properties of ternary Al-Mo-Ni alloys has been discussed [1987San]. Convergent-beam electron diffraction has been used by [1986Kau] to reveal local lattice distortions in directionally
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
5
6
9
Al–Mo–Ni
solidified γ´, Ni3Al type alloys with 12.8 at.% Al and 22.2 at.% Mo. TEM data [1990Yam] from a Mo20Ni75Al5 alloy annealed at 800˚C and quenched revealed the close-packed planes of the γ´´ and γ´ phases to be parallel: [100]γ´//[110]γ´, (010)γ´´//(111)γ´ and [001]γ//[112]γ´. [2001Kai] studied the effect of molybdenum on the morphological stability of the interface between the γ´ and β phases using Al-Mo-Ni ternary diffusion couples annealed at temperatures ranging from 900 to 1300˚C. Nonplanar interfaces with the Widmanstaetten-like structure were formed in the couples.
. Table 1 Crystallographic Data of Solid Phases Phase/ Temperature Range [˚C] (Al) < 660.452
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm] cF4 Fm 3m Cu
a = 404.88
cI2 Im 3m W
a = 314.7
pure Mo, at 25˚C [V-C]
a = 314.6 a = 314.5
x = 0, y = 0.004 [1980Fer] x = 0, y = 0.009 [1980Fer] y = 0, x = 0 to 0.035, at 1000˚C [1967Bel] y = 0, x = 0 to 0.055, at 1205˚C [1951Ham] y = 0, x = 0 to 0.068, at 1316˚C [1951Ham] y = 0, x = 0 to 0.077, at 1317˚C [1951Ham] y = 0, x = 0 to 0.096, at 1482˚C [1951Ham] y = 0, x = 0 to 0.11, at 1572˚C [1982Shi] y = 0, x = 0 to 0.108, at 1600˚C [1971Rex] y = 0, x = 0 to 0.114, at 1604˚C [1982Shi] y = 0, x = 0 to 0.14, at 1700˚C [1971Rex] y = 0, x = 0 to 0.138, at 1748˚C [1982Shi] y = 0, x = 0 to 0.195, at 2150˚C [1951Ham]
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
pure Al at 24˚C [V-C]
x = 0, y = 0 to 0.004 [2004Sal] y = 0, x = 0 to 0.00028 at 400˚C [1960Vig] y = 0, x = 0 to 0.00062 at 640˚C [1960Vig] y = 0, x = 0 to 0.0007 at 640˚C, by extrapolation [1960Vig]
MoxNiyAl1–x–y
α, (Mo) < 2623 α,(Mo1–x–yNiyAlx)
Comments/References
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Table 1 (continued) Phase/ Temperature Range [˚C] γ, (Ni) < 1455 γ, (MoxNi1–x)
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm] cF4 Fm3m Cu
a = 352.40 a = 352.32 a = 355.8 a = 353.9 a = 355.2 a = 356.5 a = 356.3 a = 361.0
γ, (Ni1–xAlx)
a = 352.8 a = 353.2
Comments/References pure Ni at 25˚C [1984Och2, Mas2] pure Ni at 20˚C [V-C] quenched from 800˚C [V-C] x = 0.03, quenched from 1000˚C [1984Och1, 1984Och2, 1985Mis] x = 0.06, quenched from 1000˚C [1984Och1, 1984Och2, 1985Mis] x = 0.09, quenched from 1000˚C [1984Och1, 1984Och2, 1985Mis] x = 0.097 [1980Fer] x = 0.218 [1980Fer] x = 0 to 0.2 [2004Sal] x = 0.2 at 1372˚C [2004Sal] x = 0.025 Slowly cooled alloy [1952Tay] x = 0.05 Slowly cooled alloy [1952Tay]
θ, MoNi4 < 870
tI10 I4/m MoNi4
a = 572.0 c = 356.4
[V-C]
γ´´, MoNi3 < 910
oP8 Pmmn TiCu3
a = 506.4 b = 422.2 c = 444.8
[V-C]
δ, MoNi < 1362
oP112 Cmcm MoNi
(Mo,Ni,Al)1 (Ni,Mo,Al)1
a = 910.8 b = 910.8 c = 885.2 a = 455 b = 1663 c = 873
46 to 48 at.% Ni [Mas2] at 50.8 at.% Ni [1980Fer]
[1997Jin]
0 to 2 at.% Al [1969Vir] 0 to 1.6 at.% Al, T = 1260˚C [1984Mir] 0 to 1.2 at.% Al, T = 1200˚C [1988Mas] 0 to 1.1 at.% Al, T = 1171˚C [1984Mir] 0 to 1.1 at.% Al, T = 1100˚C [1988Mas] 0 to 0.6 at.% Al, T = 1093˚C [1984Mir] 0 to 0.5 at.% Al, T = 1038˚C [1984Mir] 0 to 0.3 at.% Al, T = 927˚C [1984Mir] MoAl12 < 712
Landolt‐Bo¨rnstein New Series IV/11E1
cI26 Im3 WAl12
a = 757.3 a = 758.15
MSIT1
92.4 at.% Al [1991Sch] [1954Ada] [1980Fer]
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
7
8
9
Al–Mo–Ni
. Table 1 (continued) Phase/ Temperature Range [˚C] MoAl5 (h2) 846 to 800 - 750
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm] hP12 P63 WAl5
hP60 MoAl5 (h1) 3 800 - 750 to 648 P MoAl5 (h1)
Comments/References
a = 491.2 c = 886.0 a = 489 c = 880
83.8 at.% Al [1991Sch]
a = 493.3 c = 4398
at 83.3 at.% Al [1991Sch]
a = 495.1 c = 2623
at 83.3 at.% Al [1991Sch]
[1980Fer]
MoAl5 (r) ≲ 648
hP36 R3c MoAl5 (r)
Mo5Al22 964 to 831
oF216 Fdd2 Mo5Al22
Mo4Al17 < 1034
mC84 C2 Mo4Al17
MoAl4 1177 to 942
mC30 Cm WAl4
Mo1–xAl3+x 1260 to 1154
cP8 Pm 3n Cr3Si
MoAl3 1222 to 818
mC32 C2/m MoAl3
a = 1639.6 ± 0.1 b = 359.4 ± 0.1 c = 838.6 ± 0.4 β = 101.88 ± 0.07
Mo3Al8 < 1555 ± 10
mC22 Cm Mo3Al8
72 to 75 at.% Al [Mas2] a = 920.8 ± 0.3 [1962For] b = 363.78 ± 0.03 c = 1006.5 ± 0.3 β = 100.78 ± 0.05˚
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
a = 7382 ± 3 b = 916.1 ± 0.3 c = 493.2 ± 0.2 a = 915.8 ± 0.1 b = 493.23 ± 0.08 c = 2893.5 ± 0.5 β = 96.71 ± 0.01
81.7 at.% Al [1991Sch] [1995Gri]
80.9 at.% Al [1991Sch] [1995Gri]
79 to 80 at.% Al [1991Sch] a = 525.5 ± 0.5 [1964Lea] b = 1776.8 ± 0.5 c = 522.5 ± 0.5 β = 100.88 ± 0.06˚ a = 525.5 [1991Sch] b = 1176.8 c = 522.5 β = 100.7˚ a = 494.5 ± 0.1
MSIT1
76 to 79 at.% Al [1991Sch] [1991Sch] at 75 at.% Al [1991Sch]
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Table 1 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm]
Comments/References
Mo2Al3 1570 to 1490
-
-
MoAl 1750 to 1470
cP2 Pm 3m CsCl
46 to 51.7 at.% Al [Mas2] Called “ζ2” (h) [1971Rex] a = 309.8 [1971Rex] a = 309.8 to 309.9 [1980Fer]
Mo3Al ≲ 2150 (Mo,Ni,Al)3 (Al,Mo,Ni)1
cP8 Pm3n Cr3Si
ε, NiAl3 < 856
oP16 Pnma NiAl3
oP16 Pnma Fe3C Ni2Al3 < 1138
β´, Ni3Al4 < 702
Landolt‐Bo¨rnstein New Series IV/11E1
hP5 P3m1 Ni2Al3
cI112 Ia3d Ni3Ga4
Called “ζ1” (h) [1971Rex]
a = 495 a = 487.6 a = 661.15 b = 736.64 c = 481.18 a = 661.3 ± 0.1 b = 736.7 ± 0.1 c = 481.1 ± 0.1 a = 659.8 b = 735.1 c = 480.2 a = 403.63 c = 490.65 a = 402.8 c = 489.1 a = 1140.8 ± 0.1
MSIT1
22 to 27 at.% Al [Mas2] [1958Woo] at 6 at.% Ni, 75 at.% Mo [1969Vir] [L-B]
[1996Vik]
[1997Bou, V-C]
36.8 to 40.5 at.% Al [Mas2] [L-B] [1997Bou, V-C] [1989Ell, V-C]
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
9
10
9
Al–Mo–Ni
. Table 1 (continued) Phase/ Temperature Range [˚C] β, NiAl < 1651
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm] cP2 Pm 3m CsCl
a = 287.04 a = 287.26 a = 286.0 a = 287.0 a = 288.72 ± 0.02 a = 287.98 ± 0.02 a = 289.0 a = 289.7 a = 290.4 a = 291.2 a = 291.9 a = 293.2
(Ni,Mo,Al)1 (Al,Mo,Ni)1
Ni5Al3 < 723
oC16 Cmmm Pt5Ga3
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
Comments/References 42 to 69.2 at.% Ni [Mas2] 57.7 at.% Ni [L-B] 46.6 at.% Ni [L-B] [1987Kha] 63 at.% Ni [1993Kha] 50 at.% Ni [1996Pau] 54 at.% Ni [1996Pau] [1971Cli]: T = 0˚C T = 200˚C T = 400˚C T = 600˚C T = 800˚C T = 1000˚C 0 to 1.5 at.% Mo, T = 1200˚C [1983Nas] 0 to 0.3 at.% Mo, T = 1200˚C [1988Mas] 0 to 0.2 at.% Mo, T = 1100˚C [1988Mas] 0 to 4.0 at.% Mo, T = 1093˚C [1984Mir] 63 to 68 at.% Ni [1993Kha, Mas2] at 63 at.% Ni [1993Kha]
a = 753 b = 661 c = 376
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Table 1 (continued) Phase/ Temperature Range [˚C] γ´, Ni3Al < 1372
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm] cP4 P m3m Cu3Au
Ni3(Al1–xMox)
a = 356.6 a = 357.0 a = 356.77 a = 356.32 a = 357.92 a = 356.7
a = 357.0 a = 357.8 a = 356.8 a = 357.2
Ni2Al9
Landolt‐Bo¨rnstein New Series IV/11E1
mP22 P21/c Ni2Al9
a = 868.5 ± 0.6 b = 623.2 ± 0.4 c = 618.5 ± 0.4 β = 96.50 ± 0.05˚
MSIT1
Comments/References 73 to 76 at.% Ni [Mas2] [1952Tay] [1984Och2, 1959Gua1] [1986Hua] disordered [1998Rav] ordered [1998Rav] at x = 0 [1963Arb] As scaled from diagram, linear da/dx, alloys quenched from 1000˚C [1984Och1, 1984Och2, 1985Mis]: at x = 0 at 4 at.% Mo, 75 at.% Ni at 1.5 at.% Mo, 75 at.% Ni [1963Arb] at 1.5 at.% Mo, 73.5 at.% Ni [1963Arb] 0 to 4 at.% Mo, T = 1260˚C [1984Mir] 0 to 4.6 at.% Mo, at 1200˚C [1988Mas] 0 to 4.8 at.% Mo, at 1171˚C [1984Mir] 0 to 4.9 at.% Mo, at 1100˚C [1988Mas] 0 to 5.7 at.% Mo, at 1038 - 1093˚C [1984Mir] 0 to 5 - 6 at.% Mo, at 1000˚C [1977Aig, 1983Och, 1983Nas, 1984Och1, 1984Och2, 1984Mir, 1985Nas, 1985Mis, 1988Mas, 1989Hon1, 1989Mas, 1993Kub] 0 to 5.9 at.% Mo, at 927˚C [1984Mir] Metastable; [1988Li, 1997Poh]
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
11
12
9
Al–Mo–Ni
. Table 1 (continued) Phase/ Temperature Range [˚C] NixAl1–x 0.60 < x < 0.68
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm] tP4 P4/mmm AuCu
m**
Ni2Al
hP3 P 3m1 CdI2 aP126 P 1
a = 383.0 c = 320.5 a = 379.5 c = 325.6 a = 379.5 c = 325.6 a = 379.5 c = 325.6 a = 379.9 to 380.4 c = 322.6 to 323.3 a = 371.7 to 376.8 c = 335.3 to 339.9 a = 378.00 c = 328.00 a = 418 b = 271 c = 1448 β = 94.3˚ a = 407 c = 499 a ≈ 1252 b ≈ 802 c ≈ 1526 α ≈ 90˚ β ≈ 109.7˚ γ ≈ 90˚
Comments/References Martensite, metastable [1993Kha] 62.5 at.% Ni [1991Kim] 63.5 at.% Ni [1991Kim] 66.0 at.% Ni [1991Kim] 64 at.% Ni [1997Pot] 65 at.% Ni [1997Pot] [1998Sim] [1992Mur]
Metastable [1993Kha] [1994Mur]
D1 (Al-Ni)
decagonal
-
Metastable [1988Li]
D4 (Al-Ni)
decagonal
-
Metastable [1988Li]
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
9
Al–Mo–Ni
. Table 1 (continued) Phase/ Temperature Range [˚C] * τ1, Mo(NixAl1-x)3
Pearson Symbol/ Space Group/ Lattice Prototype Parameters [pm] tI8 I4/mmm TiAl3
a = 370.2 c = 836.1 a = 373.2 c = 843.0 a = 373 c = 1680 a = 376.1 ± 0.6 c = 841.2 ± 0.8 a = 373 c = 1680
superstructure? c = 2c0 * τ2, Mo11Ni14Al75
a = 1005.4 ± 0.4 b = 1528.8 ± 0.4 c = 851.9 ± 0.2
orthorhombic
Comments/References [1971Pry], at 3 to 8 at.% Ni 25 at.% Mo, 600˚C at 1.6 to 6.0 at.% Ni [2002Gru] Called “Mo2NiAl5” [1965Ram], from a threephase alloy Mo25Ni25Al50 at ≈4 to 12 at.% Ni, 25 at.% Mo, 900˚C [1969Vir] From a three-phase alloy Mo25Ni17Al58 [1969Vir] Called “N” [2002Gru] for Mo(Al2,75Ni0,25) [1969Rec] from aluminothermic synthesis Called “X” [2002Gru] Called “Mo5Ni18Al77” [1969Mar, 1971Pry]
. Table 2 Invariant Equilibria Composition (at.%) Reaction
T [˚C]
Type
LÐα+β
≈1600
e1 (max)
L α β
L + β Ð α + γ´
1340
U1
L α β γ´
L+δÐα+γ
L Ð α + γ + γ´
Landolt‐Bo¨rnstein New Series IV/11E1
≈1310
≈1300
U2
E
Phase
L α δ γ L α γ γ´
MSIT1
Al 45 1 48.5
Ni
10 97.5 2.5
45 1.5 49
13 95.5 1.5 2
20.5 <4 <33 <25 8.58 <0.5 <2.5 <8 18 <2 <17 <20.5
Mo
66.5 >0.5 >65.5 >73
27.22 97.5 50.5 20
64.2 >2.0 >47 >72
16 96.0 10 5.5
66 >2 >73 >74
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
13
14
9
Al–Mo–Ni
. Table 2 (continued) Composition (at.%) Reaction
T [˚C]
γ + α Ð γ´ + δ
≈1130
Type U3
Phase α δ γ γ´
Al
Mo
Ni
1 2 10 20
98.2 49 14 5
0.8 49 76 75
δ + γ Ð γ´+ γ´´
≈890
U4
δ γ γ´ γ´´
1 5.5 20.5 2.5
51 14 5.5 22.5
48 80.5 74 75
γ + γ´´ Ð γ´ + θ
≈730
U5
γ γ´ γ´´ θ
5.5 20 3 1
11.5 5 22 19
83 75 75 80
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Fig. 1 Al-Mo-Ni. Partial quasibinary system Mo-NiAl
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
15
9
Al–Mo–Ni
. Fig. 2 Al-Mo-Ni. Reaction scheme of the partial Mo-NiAl-Ni system
16
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Fig. 3 Al-Mo-Ni. Liquidus surface in the Ni-rich region
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
17
18
9
Al–Mo–Ni
. Fig. 4 Al-Mo-Ni. Partial isothermal section at 1260˚C
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Fig. 5 Al-Mo-Ni. Isothermal section at 1200˚C, calculated by [1974Kau]
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
19
20
9
Al–Mo–Ni
. Fig. 6 Al-Mo-Ni. Partial isothermal section at 1100˚C
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Fig. 7 Al-Mo-Ni. Partial isothermal section at 1000˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
21
22
9
Al–Mo–Ni
. Fig. 8 Al-Mo-Ni. Partial isothermal section at 1038˚C in the Al-poor region and at 1050˚C in the Al-rich region
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Fig. 9 Al-Mo-Ni. Partial isothermal section at 927˚C in the Al-poor region and at 950˚C in the Al-rich region
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
23
24
9
Al–Mo–Ni
. Fig. 10 Al-Mo-Ni. Partial isothermal section at 880˚C
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
. Fig. 11 Al-Mo-Ni. Partial isothermal section at 700˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
25
26
9
Al–Mo–Ni
. Fig. 12 Al-Mo-Ni. Partial isopleth at 14 at.% Al
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni
9
References [1925Pfa] [1933Roe] [1951Ham] [1952Tay] [1954Ada] [1958Woo]
[1959Gua1] [1959Gua2] [1960Bag] [1960Vig]
[1962For] [1963Arb]
[1964Lea] [1965Ram]
[1967Bel]
[1969Mar]
[1969Rec]
[1969Vir] [1970Cli] [1971Cli]
[1971Nal]
Pfautsch, H., “The System Aluminium-Molybdenum-Nickel” (in German), Z. Metallkd., 19(4), 125–127 (1925) (Experimental, Phase Diagram, 8) as quoted by [1993Kub] Roentgen, P., Koch, W., “Influence of Heavy Metals on Alloys of Aluminium” (in German), Z. Metallkd., 25, 182–185 (1933) (Experimental, 8) Ham, J.L., “An Introduction to Arc-Cast Molybdenum and its Alloys”, Trans. Amer. Soc. Mech. Eng. (ASME), 73, 723–732 (1951) (Experimental, 10) as quoted by [2005Sch] Taylor, A., Floyd, R.W., “The Constitution of Nickel-Rich Alloys of the Nickel-Chromium-Aluminium System”, J. Inst. Met., 81, 451–464 (1952–1953) (Experimental, Crys. Structure, Phase Diagram, 15) Adam, J., Rich, J.B., “The Crystal Structure of WAl5”, Acta Crystallogr., 7, 813–816 (1954) (Experimental, Crys. Structure, 14) Wood, E.A., Compton, V.B., Matthias, B.T., Corenzwit, E., “β-Wolfram Structure of Compounds Between Transition Elements and Aluminium, Gallium and Antimony”, Acta Crystallogr., 11, 604–606 (1958) (Experimental, Crys. Structure, 13) Guard, R.W., WestBrook, J.H., “Alloying Behavior of Ni3Al (γ´ phase)”, Trans. Met. Soc. AIME, 215, 807–814 (1959) (Phase Diagram, Experimental, 27) Guard, R.W., Smith, E.A., “Constitution of Nickel-Base Ternary Alloys”, J. Inst. Met., 88, 283–287 (1959–1960) (Phase Diagram, Experimental, 3) Bagaryatskiy, Y.A., Ivanovskaya, L.E., “Equilibrium Diagram for Ni-NiAl-Mo Alloys” (in Russian), Dokl. Akad. Nauk SSSR, 132, 339–342 (1960) (Experimental, Phase Diagram, 14) Vigdorovich, V.N., Glazov, V.M., Glagoleva, N.N., “Investigation of the Solubility of Cr, Mo and W in Al by the Microhardness Method” (in Russian), Izv. Vyss. Uchebn. Zaved., Tsvet. Met., 3(2), 143–146 (1960) (Experimental, Phase Diagram, 16) Forsyth, J.B., Gran, G., “The Structure of the Intermetallic Phase γ (Mo-Al)-Mo3Al8”, Acta Crystallogr., 15, 100–104 (1962) (Experimental, Crys. Structure, 13) Arbuzov, M.P., Zelenkov, I.A., “Structure of Ni3Al Alloys with Additions of a Third Element”, Phys. Met. Metallogr., 15(5), 71–73 (1963), translated from Fiz. Met. Metalloved., 15(5), 725–728 (1963) (Crys. Structure, Experimental, 6) Leake, J.A., “The Refinement of the Crystal Structure of the Intermetallic Phase Al4Mo”, Acta Crystallogr., 17, 918–924 (1964) (Experimental, Crys. Structure, 38) Raman, A., Schubert, K., “On the Constitution of Alloys Related to TiAl3, III. Investigations in Some T-Ni-Al and T-Cu-Al Systems” (in German), Z. Metallkd., 56, 99–104 (1965) (Crys. Structure, Experimental, 14) Belyaeva, G.I., Ilyushchenko, N.G., Anfinogenov, A.I., “Thermodynamics of Solid Alloys of a Mo-Al System” (in Russian), Tr. Inst. Electrochim. Akad. Nauk SSSR, (10), 85–95 (1967) (Experimental, Thermodyn., 25) Markiv, V.Ya., Burnashova, V.V., Pryakhina, L.L., Myasnikova, K.P., “Phase Equilibria in the Mo-Ni-Al System”, Russ. Metall., (5), 117–119 (1969), translated from Izv. Akad. Nauk SSSR, Met., (5), 180 (1969) (Phase Diagram, Experimental, 14) Rechkin, V.N., Samsonova, T.I., “Production of Mo-Ni-Al Alloys by Aluminothermic Reaction”, Russ. Metall., (3), 61–63 (1969), translated from Izv. Akad. Nauk SSSR, Met., (3), 61–64 (1969) (Crys. Structure, Experimental, 7) Virkar, A.V., Raman, A., “Alloy Chemistry of τ (βU)-Related Phases”, Z. Metallkd., 60, 594–600 (1969) (Phase Diagram, Crys. Structure, Experimental, 25) Cline, H.E., Walter, J.L., “The Effect of Alloy Additions on the Rod-Plate Transition in the Eutectic NiAl-Cr”, Metall. Trans., 1, 2907–2917 (1970) (Phase Diagram, Experimental, 20) Cline, H.E., Walter, J.L., Koch, E.F., Osika, L.M., “The Variation of Interface Dislocation Networks with Lattice Mismatch in Eutectic Alloys”, Acta Metall., 19, 405–414 (1971) (Experimental, Crys. Structure, 14) Nalibaev, T.N., Fasman, A.B., Inayatov, N.S., “Structure of Multicomponent Foraminate Catalysts Based on Nickel”, Russian J. Phys. Chem., 45, 211–214 (1971), translated from Zh. Fiz. Khim., 45, 383–386 (1971) (Experimental, 8)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
27
28
9 [1971Pry]
[1971Rex] [1973Wal] [1974Kau] [1974Tho] [1976Hen] [1976Jac]
[1976Mon] [1976Nes]
[1976Spr] [1977Aig]
[1977Pea]
[1978Gul]
[1980Fer]
[1981Sch]
[1982Shi] [1983Nas] [1983Och] [1983Wak]
[1984Kov1]
[1984Kov2] [1984Mir]
Al–Mo–Ni Pryakhina, L.I., Myasnikova, K.P., Markiv, V.Ya., Burnasheva, V.V., “Investigation of the MolybdenumNickel-Aluminium Ternary System” in “Phase Diagrams of Metal Systems” (in Russian), Nauka, Moscow, 112–116 (1971) (Phase Diagram, Experimental, 4) Rexer, J., “Phase Equilibria in the System Al-Mo at Temperatures above 1400˚C” (in German), Z. Metallkd., 62, 844–848 (1971) (Experimental, Crys. Structure, Phase Diagram, 23) Walter, J.L., Cline, H.E., “Stability of the Directionally Solidified Eutectics NiAl-Cr and NiAl-Mo”, Metall. Trans., (4), 33–38 (1973) (Experimental, 10) Kaufman, L., Nesor, H., “Calculation of Superalloy Phase Diagrams, Part II”, Metall. Trans., 5, 1623–1629 (1974) (Phase Diagram, Thermodyn., 20) Thompson, E.R., Lemkey, F.D., “Metallic Matrix Composites”, Kreider, K.G. (Ed.), Academic Press, New York, 101 (1974) as quoted by [1983Nas] Henry, M.F., “Precipitation of γ’ in γ-α (Ni-Al-Mo) Eutectics”, Scr. Metall., 10, 955–957 (1976) (Phase Diagram, Experimental, 3) Jackson, M.R., Walter, J.L., “Superalloy Eutectic Composites with the VIA Refractory Elements - Cr, Mo, W”, Superalloys-Metallurgy and Manufacture, AIME, N.Y., 341–350 (1976) (Review, Phase Diagram, 42) Mondolfo, L.F., “Aluminium Alloys: Structure and Properties”, Butterworths, London, 598–599 (1976) (Review, 5) as quoted by [1993Kub] Nesterovich, L.N., Kupchenko, G.V., Ivanov, N.P., Budnikov, V.T., “Structure and Properties of Some Directionally Crystallized Eutectics Based on Nickel”, Phys. Met. Metallogr., 42, 117–123 (1976), translated from Fiz. Metall. Metalloved., 42, 1034–1041 (1976) (Phase Diagram, Experimental, 11) Sprenger, H., Richter, H., Nickel, J.J., “Directional Solidification of Ni-Mo-Al Eutectic Alloys”, J. Mater. Sci., 11, 2075–2081 (1976) (Phase Diagram, Experimental, 17) Aigeltinger, E.R., Bates, S.R., Gould, R.W., Hren, J.J., Rhines, F.N., “Phase Equilibria in Rapidly Solidified Nickel-Rich Ni-Mo-Al Alloys”, Proc. Internat. Conf. Rapid Solidification Processing. Principles and Technologies, Reston, Virginia, Claitor’s Publishing Div., Baton Rouge, 291–305 (1977), (Publ. 1978) (Phase Diagram, Crys. Structure, Experimental, Review, 20) as quotet by [1993Kub] Pearson, D.D., Lemkey, F.D., “Solidification and Properties of γ/γ´-αMo Ductile/Ductile Eutectic Superalloy”, Proc. Conf. Solidification and Casting of Metals, Metals Soc. London, Sheffield, U.K., 526–532 (1977) (Publ. 1979) (Phase Diagram, Experimental, 18) as quoted by [1993Kub] Gulyaev, B.B., Grigorash, E. F., Efimova, M. N., “Solidification Range of Nickel Alloys”, Heat-Resistant Steels and Alloys, (11), 914–917 (1978) translated from Metallov. Term. Obrab. Met., 11, 34–37 (1978) (Experimental, Phase Diagram, 8) Ferro, R., Marazza, R., “Crystal Structure and Density Data, Molybdenum Alloys and Compounds other than Halides and Chalcogenides”, Atomic Energy Rev.: Spec. Iss. No.7, IAEA, Vienna (1980) (Crys. Structure, Review, 961) Schwam, D., Dirnfeld, S.F., “Influence of Solidification Parameters on Microstructure of γ/γ’-α(Mo) Eutectic Alloy”, Conf. Mater. Eng., Freund Publ. House Tel Aviv, 1981, 10–13 (1981) (Phase Diagram, Experimental, 7) as quoted by [1993Kub] Shilo, I., Franzen, H.F., “High Temperature Thermodynamic Study of the Molybdenum-Rich Regions of the Mo-Al System”, J. Electrochem. Soc., 129, 2613–2617 (1982) (Experimental, Thermodyn., 13) Nash, P., Fielding, S., West, D.R.F., “Phase Equilibria in Nickel-Rich Ni-Al-Mo and Ni-Al-W Alloys”, Met. Sci., 17(4), 192–194 (1983) (Phase Diagram, Experimental, #, 20) Ochiai, S., Oya, Y., Suzuki, T., “Solubility Data in Ni3Al with Ternary Additions”, Bull. P.M.E. (T.I.T.), 52, 1–16 (1983) (Phase Diagram, Review, Experimental, 4) Wakashima, K., Hoguchi, K., Suzuki, T., Umekawa, S., “Reinvestigation of Phase Equilibria in the System Ni-Al-Mo and its Implication to the Elevated Temperature Stability of γ/γ’ α-Mo Aligned Eutectics”, Acta Metall., (11), 1937–1944 (1983) (Phase Diagram, Experimental, 19) as quoted by [1993Kub] Kovacova, K., Kristin, J., “Morphological Properties of γ/γ’-αMo Eutectic Composite Material” (in Czech), Kovove Mater., 22(3), 347–356 (1984) (Phase Diagram, Experimental, 18) as quoted by [1993Kub] Kovacova, K., “Undirectional Solidification of Ni-Al-Mo Alloy”, J. Cryst. Growth, 66, 426–430 (1984) (Phase Diagram, Experimental, 9) Miracle, D.B., Lark, K.A., Srinivas, V., Lipsitt, H.A., “Nickel-Aluminium-Molybdenum Phase Equilibria”, Metall. Trans. A, 15A, 481–486 (1984) (Phase Diagram, Experimental, #, 12)
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni [1984Och1] [1984Och2] [1984Sch] [1985Mis]
[1985Nas]
[1986Hor]
[1986Hua] [1986Kau]
[1986Mas1]
[1986Mas2]
[1987Kha] [1987San]
[1987Sve]
[1988Li]
[1988Mas]
[1989Ell] [1989Gai]
[1989Hon1] [1989Hon2] [1989Mas] [1990Yam]
9
Ochiai, S., Oya, Y., Suzuki, T., “Alloying Behavior of Ni3Al, Ni3Ga, Ni3Si and Ni3Ge”, Acta Metall., 32, 289–298 (1984) (Phase Diagram, Experimental, 90) Ochiai, S., Mishima, Y., Suzuki, T.S., “Lattice Parameter Data of Ni(γ), Ni3Al (γ’) and Ni3Ga (γ’) Solid Solutions”, Bull. P.M.E. (T.I.T.), 53, 15–28 (1984) (Crys. Structure, Experimental, 66) Schwam, D., Dirnfeld, S.F., Nadiv, S., “Microstructural Instability of Ni-Mo-Al Unidirectionally Solidified Eutectics”, J. Mater. Sci. Lett., (3), 363–366 (1984) (Experimental, Crys. Structure, 6) Mishima, S., Ochiai, S., Suzuki, T.Y., “Lattice Parameters of Ni (γ), Ni3Al (γ’) and Ni3Ga (γ’) Solid Solutions with Additions of Transition and B-Subgroup Elements”, Acta Metall., 33, 1161–1169 (1985) (Crys. Structure, Experimental, 64) Nash, P., “Ni-Base Intermetallics for High Temperature Alloy Design “High-Temperature Ordered Intermetallic Alloys”, Mater. Res. Soc. Symposia Proceedings, Kreh, C.C., Liu, C.T., Stoloff, N.S., (Eds.), MRS-Pennsylvania, Boston, Massachusetts (1984), 39, 423–427 (1985) (Phase Diagram, Review, 15) Horita, Z., Sano, T., Nemoto, M., “Identification of Fine Particles in Unidirectionally Solidified Ni-AlMo Eutectic Alloys by Means of EDX and SAD Analyses”, Acta Metall., 34(8), 1525–1531 (1986) (Experimental, Crys. Structure, *, 27) Huang, S.C., Briant, C.L., Chang, K.-M., Taub, A.I., Hall, E.L., “Carbon Effects in Rapidly Solidified Ni3Al”, J. Mater. Res., 1(1), 60–67 (1986) (Experimental, Mechan. Prop., 27) Kaufman, M.L., Pearson, D.D., Fraser, H.L., “The Use of Convergent beam Electron Diffraction to Determine Local Lattice Distortions in Nickel Base Superalloys”, Philos. Mag., A54, 79–92 (1986) (Crys. Structure, Experimental, 11) Maslenkov, S.B., Udovskii, A.L., Burova, N.N., Rodimkina, V.A., “Phase Diagram of the NickelAluminium-Molybdenum System at 1300–2000˚C”, Russ. Metall., (1), 203–209 (1986), translated from Izv. Akad. Nauk SSSR, Met., (1), 198–205 (1986) (Phase Diagram, Experimental, 9) Maslenkov, S.B., Rodimkina, V.A., “Phase Equilibrium of the System Ni-Al-Mo in the Composition Range Ni-NiAl-Mo”, Russ. Metall., (3), 215–220 (1986), translated from Izv. Akad. Nauk SSSR, Met., (3), 218–223 (1986) (Phase Diagram, Experimental, 7) Khadkikar, P.S., Vedula, K., “An Investigation of the Ni5Al3 Phase”, J. Mater. Res., 2(2), 163–167 (1987) (Experimental, Crys. Structure, 7) Sano, T., Nemoto, M., “Precipitates in Nickel-Rich Ni-Al-Mo Ternary Alloys”, Trans. Jpn. Inst. Met., 28, 8–19 (1987), translated from J. Jpn. Inst. Met., 49(8), 690–698 (1985) (Crys. Structure, Experimental, 52) Svetlov, I.L., Udovski, A.L., Monastyrskaya, E.V., Oldakovskii, I.V., Nazarova, M.P., “Calculation of the Monovariant Liq/(Liq + γ + α) Line in the Ni-Mo-Al System and Plane Front Solidification in γ/γ´ - α Alloys”, Russ. Metall., (6), 186–192 (1987), translated from Izv. Akad. Nauk SSSR, Met., (6), 183–189 (1987) (Phase Diagram, 14) Li, X.Z., Kuo, K.H., “Decagonal Quasicrystals with Different Peridicities Along the Tenfold Axis in Rapidly Solidified Al-Ni Alloys”, Phil. Mag. Lett., 58(3), 167–171 (1988) (Experimental, Crys. Structure, 14) Maslenkov, S.B., Burova, N.N., Rodimkina, V.A., “The Ni-NiAl-Mo State Diagram in the 1200–700˚C Temperature Range” (in Russian), Izv. Akad. Nauk SSSR, Met., (6), 183–190 (1988) (Phase Diagram, Experimental, #, 13) Ellner, M., Braun, J., Predel, B., “X-Ray Diffraction Investigation of Al-Cr Phases of the W Family” (in German), Z. Metallkd., 80, 374–383 (1989) (Experimental, Crys. Structure, 38) Gaidukov, A.M., Udovskii, A.L., Oldakovski, I.V., “Construction of Mathematical Models in the Liquid System Surface” (in Russian), Dokl. Akad. Nauk SSSR, 305, 643–648 (1989) (Review, Theory, 15) Hong, Y.M., Nakajima, H., Mishima, Y., Suzuki, T., “The γ Solvus Surface in Ni-Al-X (X = Cr, Mo and W) Ternary Systems”, ISIJ International, 29(1), 78–84 (1989) (Phase Diagram, Experimental, #, 25) Hong, Y.M., Mishima, Y., Suzuki, T., “Accurate Determination of γ’ Solvus in Ni-Al-X Ternary Systems”, Mater. Res. Soc. Symp. Proc., 733, 431–438 (1989) (Phase Diagram, Experimental, 35) Maslenkov, S.B., Rodimkina, V.A., “Phase Changes in Alloys of the System Ni-NiAl-Mo” (in Russian), Izv. Akad. Nauk SSSR, Met., (1), 194–198 (1989) (Phase Diagram, Crys. Structure, #, 12) Yamamoto, M., Iada, J., Nenno, S., “The Microstructure of a Two-Phase Mixture in a Ni75Mo20Al5 Alloy”, J. Mater. Sci. Lett., 9, 34–35 (1990) (Crys. Structure, Experimental, 5)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
29
30
9 [1991Eno]
[1991Kim]
[1991Mis] [1991Sas]
[1991Sch] [1992Mur]
[1993Kha] [1993Kub]
[1994Mur] [1995Gri] [1996Pau] [1996Vik] [1997Bou] [1997Jin] [1997Poh] [1997Pot]
[1998Mur] [1998Rav]
[1998Sim]
[1999Kau]
[1999Lu] [2000Bor]
Al–Mo–Ni Enomoto, M., Harada, H., Yamazaki, M., “Calculation of γ´/γ Equilibrium Phase Compositions in Nickel-Base Superalloys by Cluster Variation Method”, Calphad, 15(2), 143–158 (1991) (Assessment, Calculation, Phase Diagram, 34) Kim, Y.D., Wayman, C.M., “Transformation and Deformation Behavior of Thermoelastic Martensite Ni-Al Alloys Produced by Powder Metallurgy Method” (in Korean), J. Korean Inst. Met. Mater., 29(9), 960–966 (1991) (Mechan. Prop., Experimental, 15) as quoted by [2004Sal] Mishima, Y., Hong, Y.M., Suzuki, T., “Determination of the γ Solvus Surface in Ni-Al-X Ternary Systems”, Mater. Sci. Eng. A, 146, 123–130 (1991) (Assessment, Phase Diagram, Experimental, 5) Sasaki, K., Morinaga, M., Yukawa, N., “Alloying Effect on the Solidified Structure of NiAl”, Proc. Conf. Intermetal. Comp. - Struct. Mechan. Prop., 877–881 (1991) (Abstract, Phase Diagram, Experimental, Mechan. Prop., 10) Schuster, J.C., Ipser, H., “The Al-Al8Mo3 Section of the Binary System Aluminium- Molydenum”, Met. Trans., A22, 1729–1736 (1991) (Experimental, Crys. Structure, Phase Diagram, 20) Murakami, Y., Otsuka, K., Hanada, S., Watanabe, S., “Crystallography of Stress-Induced B2Ð7R Martensitic Transformation in a Ni-37.0 at.% Al Alloy”, Mater. Trans. JIM, 33(3), 282–288 (1992) (Crys. Structure, Experimental, 25) Khadkikar, P.S., Locci, I.E., Vedula, K., Michal, G.M., “Transformation to Ni5Al3 in a 63.0 At. Pct Ni-Al Alloy”, Metall. Trans. A, 24A, 83–94 (1993) (Phase Diagram, Crys. Structure, Experimental, 28) Kubaschewski, O., “Al-Mo-Ni (Aluminium - Molybdenum - Nickel),” MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.12789.1.20, (1993) (Crys. Structure, Phase Diagram, Assessment, 54) Murthy, A.S., Goo, E., “Triclinic Ni2Al Phase in 63.1 at.% NiAl”, Met. Mater., A, 25A(1), 57–61 (1994) (Crys. Structure, Experimental, 10) Grin, Y.N., Ellner, M., Peters, K., Schuster, J.C., “The Crystal Structures of Mo4Al17 and Mo5Al22”, Z. Kristallogr., 210, 96–99 (1995) (Experimental, Crys. Structure, 11) Paufler, P., Faber, J., Zahn, G., “X-Ray Single Crystal Diffraction Investigation on Ni1+xAl1-x”, Acta Crystallogr., Sect. A: Found. Crystallogr., A52, C319 (1996) (Crys. Structure, Experimental, Abstract, 3) Viklund P., Haeussermann, U., Lidin, S., “NiAl3: a Structure Type of its Own?”, Acta Crystallogr., Sect. A: Found Crystallogr., A52, C321 (1996) (Crys. Structure, Experimental, Abstract) Bouche, K., Barbier, F., Coulet, A., “Phase Formation During Dissolution of Nickel in Liquid Aluminium”, Z. Metallkd., 88(6), 446–451 (1997) (Thermodyn., Experimental, 15) Jin, Y., Chaturvedi, M.C., Han, Y.F., Zhang, Y.G., “Crystal Structure of δ-NiMo Phase in a Ternary Ni-Mo-Al Alloy”, Mater. Sci. Eng. A, A225, 78–84 (1997) (Crys. Structure, Experimental, 13) Pohla, C., Ryder, P.L., “Crystalline and Quasicrystalline Phases in Rapidly Solidified Al-Ni Alloys”, Acta Mater., 45, 2155–2166 (1997) (Experimental, Crys. Structure, 48) Potapov, P.L., Song, S.Y., Udovenko, V.A., Prokoshkin, S.D., “X-Ray Study of Phase Transformations in Martensitic Ni-Al Alloys”, Metall. Mater. Trans. A, 28A, 1133–1142 (1997) (Crys. Structure, Experimental, 40) Murthy, B.S., Ranganathan, S., Int. Mater, Rev., 43(3), 101–141 (1998), as quoted by [2002Alb] Ravelo, R., Aguilar, J., Baskes, M., Angelo, J.E., Fultz, B., Holian, B.L., “Free Energy and Vibrational Entropy Difference between Ordered and Disordered Ni3Al”, Phys. Rev. B, 57(2), 862–869 (1998) (Thermodyn., Theory, Calculation, 43) Simonyan, A.V., Ponomarev, V.I., Khomenko, N.Yu., Vishnyakova, G.A., Gorshkov, V.A., Yukhvid, V.I., “Combustion Synthesis of Nickel Aluminides”, Inorg. Mater., 34(6), 558–561 (1998), translated from Neorgan. Mater., 34(6), 684–687 (1998) (Crys. Structure, Experimental, 12) Kaufman, L., Dinsdale, A.T., “Summary of the Proceedings of the CALPHAD XXVII Meeting, 17–22 May 1998, Beijing, China”, Calphad, 23(3-4), 265–303 (1999) (Assessment, Calculation, Phase Diagram, Thermodyn., #) Lu, X., Cui, Y., Jin, Z., “Experimental and Thermodynamic Investigation of the Ni-Al-Mo System”, Metall. Mater. Trans. A, 30A, 1785–1795 (1999) (Phase Diagram, Experimental, Thermodyn., #, 28) Borgenstam, A., Engstroem, A., Hoeglund, L., Agren, J., “DICTRA, a Tool for Simulation of Diffusional Transformations in Alloys”, J. Phase Equilib., 21(3), 269–280 (2000) (Calculation, Kinetics, Thermodyn.)
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–Ni [2001Ter]
[2001Kai]
[2002Alb]
[2002Gru] [2002Guo] [2004Sal]
[2005Sch]
[L-B]
[Mas2] [V-C] [V-C2]
9
Terada, Y., Ohkubo, K., Mohri, T., Suzuki, T., “Site Preference Determination in Intermetallic Compounds by Thermal Conductivity Measurement”, J. Mater. Res., 16(8), 2314–2320 (2001) (Calculation, Crys. Structure, Experimental, Thermal Conduct., 63) Kainuma, R., Ichinose, M., Ohnuma, I., Ishida, K., “Formation of γ’/β Interface Morphologies in Ni-Al-X Ternary Diffusion Couples”, Mater. Sci. Eng. A, 312, 168–175 (2001) (Phase Diagram, Experimental, Thermodyn., 21) Albiter, A., Bedolla, E., Perez, R., “Microstructure Characterization of the NiAl Intermetallic Compound with Fe, Ga and Mo Additions Obtained by Mechanical Alloying”, Mater. Sci. Eng. A, 328, 80–86 (2002) (Crys. Structure, Experimental, 14) Grushko, B., Mi, S., Highfield, J.G., “A Study of the Al-Rich Region of the Al-Ni-Mo Alloy System”, J. Alloys Compd., 334, 187–191 (2002) (Crys. Structure, Phase Diagram, Experimental, 8) Guo, J.T., Du, X.H., Zhou, L.Z., Zhou, B.D., Qi, Y.H., Li, G.S., “Superplasticity in NiAl and NiAl-Based Alloys”, J. Mater. Res., 17(9), 2346–2356 (2002) (Experimental, Mechan. Prop., 17) Saltykov, P., Cornish, L., Cacciamani, G., “Al-Ni (Aluminium-Nickel)”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services, GmbH, Stuttgart; Document ID: 20.10238.1.20, (2004) (Crys. Structure, Phase Diagram, Assessment, 164) Schuster, J.C., “Al-Mo (Aluminium - Molybdenum)”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services, GmbH, Stuttgart; Document ID: 30.12123.1.20, (2005) (Crys. Structure, Phase Diagram, Assessment, 61) Landolt-Boernstein, Numerical Data and Functional Relationships in Science and Technology (New Series). Group 3 (Crystal and Solid State Physics), Vol. 6, Eckerlin, P., Kandler, H. and Stegherr, A., Structure Data of Elements and Intermetallic Phases (1971); Vol. 7, Pies, W. and Weiss, A., Crystal Structure of Inorganic Compounds, Part c, Key Elements: N, P, As, Sb, Bi, C (1979); Group 4: Macroscopic and Technical Properties of Matter, Vol. 5, Predel, B., Phase Equilibria, Crystallographic and Thermodynamic Data of Binary Alloys, Subvol. a: Ac-Au … Au-Zr (1991); Springer-Verlag, Berlin. Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, ASM, Metals Park, Ohio (1985) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_9 ß Springer 2009
31
Al–Mo–U
10
Aluminium – Molybdenum – Uranium Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Zoya Alekseeva, updated by Kostyantyn Korniyenko
Introduction Phase relationships in the Al-Mo-U system are of great interest, above all because an alloy comprising Mo-U alloy particles dispersed in an aluminium matrix provides a candidate material for low-enriched uranium fuel with high loading. This is because a solid solution of molybdenum in (γU) possesses acceptable irradiation and mechanical properties and can be formed over a wide range of Mo concentrations. Below 560˚C, (γU) can exist only in a metastable state, as indicated by the constitution of the Mo-U binary system. Therefore, in fuel fabrication and service it is very important to retain the metastable (γU) below 560˚C [2002Lee]. Phase equilibria in the composition range U-UAl2-Mo3Al8-Mo have been studied by [1969Pet, 1971Pet] by means of physico-chemical analysis techniques. The liquidus surface, a projection of the four-phase equilibria, the UAl2-Mo3Al8 temperature-composition section and the reaction scheme involving the liquid phase were constructed; the phase compositions for ten four-phase equilibria were determined [1969Pet]. [1971Pet] presented isothermal sections at 1250, 1050 and 500˚C. Several temperature-composition sections were also reported. More recently, the attention of investigators of phase relationships in the ternary Al-Mo-U system has been concentrated mainly on the behavior of alloys that may serve as the basis of Mo-U alloy dispersion fuels [1979Sof, 1984Gom, 2002Lee, 2003Lee, 2003Ryu, 2004Lee, 2006Ryu2, 2006Wie]. Phase development in the Al rich Al-Mo-U alloys is presented in [2004Kei]. The crystal structures of phases of the Al-Mo-U system are reported in [1964Nic, 1979Sof, 1984Gom, 1994Nie, 1995Nie, 2002Lee, 2003Mir, 2003Ryu, 2004Kei, 2004Lee, 2006Ryu2, 2007Noe]. Thermodynamic properties are reported in [2003Ryu, 2006Kim, 2006Ryu1]. Publications relating to experimental studies of phase relationships, crystal structures and thermodynamics along with the techniques employed are listed in Table 1. A review of the crystal structures of the Al-Mo-U phases is presented in [1980Fer]. The character of the phase equilibria was assessed in the previous MSIT evaluation by [1993Ale]. The present report is supplemented by information from later publications, bringing together the data in accordance with the modern versions of the boundary binary phase diagrams.
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
1
2
10
Al–Mo–U
Binary Systems The Al-Mo boundary binary system is accepted from [2005Sch]. The boundary binary Al-U system is based on a critical assessment carried out by [1990Kas], reproduced in [Mas2], however, taking UAl4 as a fully ordered, strictly stoichiometric phase [2004Tou]. The Mo-U boundary binary system is accepted from [Mas2].
Solid Phases Crystallographic data on the solid unary, binary and ternary Al-Mo-U phases and their concentration and temperature ranges of stability are presented in Table 2. A noticeable solubility of Al and Mo in (U) and Al and U in (Mo) was reported by [1969Pet, 1971Pet]. There is negligible uranium solubility in the binary Al-Mo compounds. According to [1971Pet], aluminium can be substituted by molybdenum (up to 18.5 at.% of Mo at the temperatures of 1250, 1050 and 500˚C) in the UAl2 based λ2 phase. The ternary phases τ1, U9Mo16Al75 (with unknown structure - composition lies outside the studied U-U Al2-Mo3Al8-Mo range) and the τ2 Laves phase (with the MgZn2 type structure) were identified by [1969Pet, 1971Pet]. [1994Nie] and [1995Nie] found two new ternary phases (τ3, U6Mo4Al43 and τ4, UMo2Al20) from single crystal studies. Their existence was confirmed by [2007Noe], but phase equilibria involving these phases are in need of further study.
Invariant Equilibria Temperatures, reactions types and phase composition relating to invariant equilibria in the U-U UAl2-Mo3Al8-Mo region are listed in Table 3. The reaction scheme is shown in Figs. 1a and 1b. The presented data are based on [1969Pet, 1971Pet], with amendments to ensure compatibility with the accepted boundary binary systems. In Figs. 1a, 1b and Table 3, only invariant equilibria involving the liquid phase are presented. In addition to the presented reactions (Figs. 1a, 1b, Table 3), an invariant equilibrium between liquid, τ1, λ2 and UAl3 takes place at 1305˚C in the Al rich corner. This is deduced from the UAl2-Mo3Al8 temperaturecomposition section (see “Temperature-Composition Sections” chapter). A reaction scheme for the solid state was proposed in [1971Pet] but is omitted here as it is in need of revision in light of principal changes in the invariant temperatures of the Mo-U binary system. Further experimental verification of the solid state phase equilibria in the ternary Al-Mo-U system is also necessary.
Liquidus, Solidus and Solvus Surfaces Figure 2 presents the liquidus surface projection of the U-U Al2-Mo3Al8-Mo region on the basis of studies by [1969Pet], with slight corrections in accordance with the boundary binary systems, in particular in relation to the positions of the reactions p1 and p5. The isotherms positions on the (Mo) surface at the temperatures above 1600˚C contradict to the accepted Al-Mo and Mo-U binary diagrams and need further verification. They are omitted in Fig. 2. [1969Pet] also reported the compositions of solid phases taking part in the invariant DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
equilibria, and these compositions are listed in Table 3. But the solidus surface projection is not presented here because the compositions of the Al-Mo-based phases were not determined precisely making a correct representation difficult.
Isothermal Sections Figures 3, 4 and 5 show isothermal sections determined for 1250, 1050 and 500˚C, respectively, by [1971Pet]. The composition range studied was that within the region delineated by U, Mo, Mo3Al8 and UAl2. The sections are amended to ensure consistency with the boundary binary systems. A neutron diffraction study of an atomized uranium-based alloy with 10 mass% Mo (U78.4Mo21.6 in at.%) carried out by [2002Lee] showed that homogenizing annealing above 560˚C retards the decomposition of the γ phase at 400 and 500˚C, at which temperatures the phase is metastable. It was reported that in fuel with U78.4Mo21.6 alloy particles dispersed in an Al matrix, aluminium diffuses along the grain boundaries and reacts with the α phase formed from the decomposed γ phase at 400 and 500˚C. The formation of UAl3 and λ2 was observed. The formation of ternary compounds was not detected by neutron diffraction. The phase content of the U-Mo/Al dispersion fuels at temperatures of 500, 525 and 550˚C was determined by [2003Ryu, 2006Ryu2] using a diffusion couple technique. Diffusion couples based on atomized dispersion fuel with U-7 mass% Mo (U-15.7 at.% Mo) /Al were studied by [2003Mir, 2004Lee].
Temperature – Composition Sections A number of temperature-composition sections have been reported for the U-UAl2-Mo3Al8Mo region [1969Pet, 1971Pet]. Figure 6 shows the boundary (UAl2-Mo3Al8) section of the investigated part of the ternary system. It is not quasibinary (although declared by [1969Pet, 1971Pet]) because the τ1 phase, which is involved in equilibria within the section, lies outside the plane of the section. The remaining temperature-composition sections reported in [1971Pet] are presented in Figs. 7 to 13, amended to ensure agreement with the boundary binary systems. The character of phase equilibria at the Al-Mo side of the isopleth at 50 at.% Al proposed in [1971Pet] contradicts to the accepted Al-Mo diagram (the ξ1 phase does not take part in equilibria at 50 at.% Al) and therefore the corresponding part of the vertical section is plotted in Fig. 11 by dashed lines.
Thermodynamics [2003Ryu] presented results of studies on the kinetics of the growth of reaction layers. An as-cast U-10Mo (mass%) (U-21.6Mo (at.%)) ingot was heat-treated under vacuum at 900˚C for 100 h to ensure compositional homogeneity, followed by quenching to form the γ phase. This was used to make a diffusion couple with an Al sheet. Annealing of 10 vol% (U-21.6 at.% Mo)/Al dispersion fuels was carried out at temperatures from 500 to 550˚C for times between 10 min to 36 h with a view to determine the activation energy for the growth of the reaction Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
3
4
10
Al–Mo–U
layers. It was calculated using an Arrhenius plot according to two different models (277 kJ·mol–1 from the Jander’s model and 316 kJ·mol–1 from the Ginstling-Brounshtein model). The heat generation of U-Mo/Al dispersion fuels with 10–50 vol% of Mo-U fuel during a thermal cycle from room temperature to 700˚C was measured using DSC. The exothermic heat resulting from the reaction between Mo-U and the Al matrix was largest (235 kJ·kg–1) when the volume fraction of Mo-U fuel was about 30 vol%. Irradiation-enhanced interdiffusion in the diffusion zone of a U-Mo dispersion fuel in aluminium was studied in [2006Kim]. In order to analyze fuel performance accurately, a model to predict the diffusion kinetics was proposed. The authors developed a diffusion layer growth rate correlation for out-of-pile annealing tests and a similar correlation for in-reactor tests. The correlation for in-reactor tests is considerably different from that of out-of-pile tests because it contains factors that amplify diffusion kinetics by fission damage in the diffusion reaction zone. Using an appropriate computer code, fission damage factors were obtained as a function of diffusion reaction layer thickness and composition. The model correlation was established and fitted to the in-reactor data. As a result of the data fitting, the interaction layer growth rate was found to be proportional to the square root of the fission fragment damage rate and to have a temperature dependence characterized by the effective activation energy of 46 to 76 kJ·mol–1. The heats of formation of the (U1–xMox)Al3 intermetallic compound were obtained by [2006Ryu1] by measuring the reaction heats of U-Mo/Al dispersion samples using DSC. It was concluded that the heat of formation of (U1–xMox)Al3 becomes less negative as the molybdenum content increases (about –68 kJ·mol–1 and about –55 kJ·mol–1 at x = 0.15 and x = 0.225, respectively).
Notes on Materials Properties and Applications The Al-Mo-U alloys are of great practical interest as the basis of high-density U-Mo/Al dispersion fuel. Nuclear fuels can be placed into two main categories - for energy production and for production of neutrons. The alloys of the Al-Mo-U system are candidate materials for both of these fields of application [2007Noe]. Vickers microhardness of the γ phase in an U87.5Mo12.0Al0.5 (at.%) alloy that had been homogenized at 1050˚C and then reduced and quenched from 800˚C was reported in [1984Gom] as 1.78 GPa. The effects of fuel powder volume fraction and fuel particle shape on the green properties of pressed powder compacts produced from blended U-10Mo (mass%) (U-21.6Mo (at.%)) and Al powder were investigated by [2000Han]. The relative density of the compacts increased with decreasing volume fraction of fuel powder. The compressibility of compacts prepared from comminuted powder was larger than that of the compacts made from atomized powder owing to fragmentation of the comminuted particles. The green strength of the compacts made from comminuted powder was higher than that of the atomized powder compact. In the opinion of the authors, this seemed to have resulted from the smaller pore size and the larger contact area between the comminuted fuel powder and Al powder. It was suggested that an adjustment in the compacting conditions may be required in order to fabricate compacts from atomized powder having a comparable green strength. The effect of heat treatment on the thermal conductivity of U-Mo/Al alloy dispersion fuel was reported in [2003Lee]. Thermal conductivities were calculated from measured thermal diffusivities, specific heat capacities and densities, which were determined using DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
the laser flash, DSC, and Archimedes methods, respectively. The thermophysical properties were measured over a temperature range from room temperature up to 500˚C. The Mo-U alloy was annealed at between 525 and 550˚C for between 1 and 36 h. At high temperatures, the MoU particles reacted with the aluminium matrix forming reaction layers that adversely affected the thermal conductivity of the fuel core. The thermal conductivities of annealed samples appeared to decrease with increasing volume fraction of the reaction layers.
Miscellaneous The kinetics of the isothermal transformation of the γ phase in an alloy of the composition U87.5Mo12.0Al0.5 (in at.%) was investigated by [1984Gom] using dilatometry with a cooling rate from the γ phase range of 150˚C·min–1 between 700 and 500˚C. It was concluded that in comparison with the binary Mo-U system, the addition of a comparatively minor amount of the third component aluminium has a major effect on the shape of the isothermal transformation diagram, the kinetic parameters and the completeness of transformation. Precipitation of the second intermetallic λ2 phase takes place. The thermal compatibility of centrifugally atomized Mo-U alloys with aluminium was studied by [1997Lee]. The results of their investigations show that U-2 mass% Mo/Al dispersions increase in volume by 26% at 400˚C after 2000 h. This large volume change is due mainly to the formation of voids and cracks resulting from nearly complete interdiffusion of Mo-U and aluminium. No significant dimensional changes occur in the U-10 mass% Mo/Al dispersions. Interdiffusion between U-10Mo (mass%) and aluminium was found to be minimal. The different diffusion behavior is due primarily to the fact that U-10 mass% Mo (U-21.6Mo (at.%)) particles are much more supersaturated with substitutional molybdenum than U-2Mo (mass%) (U-4.8Mo (at.%)) particles. The aluminium diffuses into the U-2Mo (mass%) particles relatively rapidly along grain boundaries forming UAl3 almost fully throughout the 2000 h anneal, whereas the molybdenum supersaturation in the U-10Mo (mass%) particles inhibits the diffusion of aluminium atoms. U-10 mass% Mo displays superior thermal compatibility with aluminium compared to U-2Mo (mass%). The irradiation behavior of atomized U78.4Mo21.6 (at.%) Mo alloy aluminium matrix dispersion fuel meat at low temperature was reported by [2002Kim]. In order to examine the in-reactor behavior of very-high-density dispersion fuels for high flux performance research reactors, the U78.4Mo21.6 alloy dispersions in an aluminium matrix have been irradiated at low temperatures in the Advanced Test Reactor (ATR). The alloy fuel dispersant was produced by a centrifugal atomization process. The fuel particles had a fine and a relatively narrow fission gas bubble size distribution. In the author’s opinion, these appeared to be features in the microstructure that result from the segregation of the microstructure into molybdenum rich and depleted regions on solidification. Irradiation tests have been conducted by [2002Mey] with a view to evaluate the performance of a series of highdensity uranium-molybdenum (U-Mo) alloy aluminium matrix dispersion fuels. Fuel plates incorporating alloys with molybdenum contents in the range of 4–10 mass% were tested. As a whole, fuels with molybdenum contents of 6 mass% or higher showed stable in-reactor fission gas behavior, exhibiting a distribution of small, stable gas bubbles. The Bozzolo-FerranteSmith (BFS) method for alloys was applied by [2003Gar] to the analysis of aluminium interdiffusion in the Mo-U solid solution as a function of Mo concentration. The binary Al/U and Al/Mo system showed opposite behavior, which in the ternary case of Al/Mo-U translates into the role of regions rich in Mo acting as interdiffusion barriers to Al, in excellent Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
5
6
10
Al–Mo–U
agreement with experimental evidence. Later, an interdiffusional model for the prediction of interaction layer growth in the Al/Mo-U system using the computer codes PLACA and DPLACA simulating the behavior of a plate-type fuel containing in its core a foil of monolithic or dispersed fissile material, respectively, under normal operation conditions of a research reactor, was proposed by [2007Sob]. The PLACA code was used to simulate experimental results from planar Al/Mo-U diffusion couple studies published in the literature. DPLACA was used to simulate experiments performed with Mo-U particles dispersed in Al, with and without irradiation. Satisfactory prediction of the whole reaction layer thickness and of the individual fractions corresponding to alloy and matrix consumption was obtained. In [2006Wie], the similarity or even equivalence of the interdiffusion layer of U-Mo/Al fuel, that was found in-pile and alternatively generated by heavy ion irradiation, was shown. A similar failure under irradiation was reported.
. Table 1 Investigations of the Al-Mo-U Phase Relations, Structures and Thermodynamics Reference
Method / Experimental Technique
Temperature / Composition / Phase Range Studied
[1964Nic]
Arc melting; heat treatment; 900˚C with cooling to room temperature metallography; X-ray diffraction; electron at 4–5˚C·min–1; U rich corner, 0.75 to 2.8 microscopy at.% Mo, 2 to 8 at.% Al
[1969Pet]
Arc melting (the starting components Al - < 2623˚C; the range U-UAl2-Mo3Al8-Mo 99.99 mass%, Mo - 99.93, U - 99.9 mass%); DTA; chemical analysis; X-ray diffraction; optical microscopy
[1971Pet]
Arc melting (the starting components Al - 1250, 1050, 500˚C; U-UAl2-Mo3Al8-Mo 99.99 mass%, Mo - 99.93, U - 99.9 mass%); annealing; DTA; X-ray diffraction; optical microscopy
[1979Sof]
Arc melting; annealing; quenching; 1050–950˚C; U rich corner, 10 and 11.5 chemical analysis; EMPA; X-ray diffraction at.% Mo, up to 3 at.% Al
[1984Gom] Arc melting; annealing; reduction; quenching; X-ray diffraction; dilatometry
1050–400˚C; U87.5Mo12.0Al0.5 (at.%)
[1994Nie]
Cold pressing (the purities of starting U6Mo4Al43 components > 99.9 mass%); annealing at 800˚C for 3 weeks, single crystal growth, SEM; X-ray diffraction (Guinier camera)
[1995Nie]
Cold pressing (the purities of starting UMo2Al20 components > 99.9 mass%); annealing at 800˚C for 3 weeks, single crystal growth, SEM; X-ray diffraction (Guinier camera)
[2002Lee]
Blending, extrusion, annealing, atomization; neutron diffraction; SEM
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
800–500˚C; U78.4Mo21.6 (at.%) with Al additions
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Table 1 (continued) Reference
Method / Experimental Technique
Temperature / Composition / Phase Range Studied
[2003Mir]
Arc melting; annealing and quenching; optical microscopy; SEM; EMPA; X-ray diffraction
580˚C; diffusion couples U-7 mass% Mo (U-15.7 at.% Mo) /Al
[2003Ryu]
Vacuum induction melting; annealing; SEM; X-ray diffraction; DSC
≤ 1400˚C; dispersion fuels U-10 mass% Mo (U-21.6 at.% Mo)/Al
[2004Kei]
Arc melting; SEM
As-cast and annealed at 500˚C alloys U0.8Mo0.2Al6 and U0.8Mo0.2Al7
[2004Lee]
Irradiation cycles (FUTURE irradiation rig of the BR2 reactor; optical microscopy; EMPA; wavelength dispersive X-ray analysis (WDX); SEM; X-ray diffraction
Low-enriched uranium fuel plates U7 mass% Mo (U-15.7 at.% Mo) atomized powder dispersed in Al matrix
[2006Kim]
SEM; EMPA
≤ 600˚C; dispersion fuels U-10 mass% Mo (U-21.6 at.% Mo)/Al
[2006Ryu1] DSC; SEM
≤ 677˚C; U-6 mass% Mo (U-13.7 at.% Mo)/ Al and U-10 mass% Mo (U-21.6 at.% Mo)/ Al dispersion samples
[2006Ryu2] Irradiation tests (HANARO reactor); X-ray diffraction; SEM; EDX
500–580˚C; U-6 to 10 mass% Mo (U-13.7 to 21.6 at.% Mo)/ (0.1 to 1.0 mass% Al) dispersion fuels
[2006Wie]
Heavy ion irradiation tests; optical microscopy; SEM; EDX; X-ray diffraction
U-6 mass% Mo (U-13.7 at.% Mo)/Al and U-10 mass% Mo (U-21.6 at.% Mo)/Al dispersion samples
[2007Noe]
EDX; X-ray diffraction
Phase equilibria with participation of the τ3 and τ4 phases
. Table 2 Crystallographic Data of Solid Phases Phase/ Temperature Range [˚C] (Al) < 660.452 UxMoyAl1–x–y
Landolt‐Bo¨rnstein New Series IV/11E1
Pearson Symbol/ Lattice Space Group/ Parameters Prototype [pm] cF4 Im3m Cu
a = 404.96
Comments/References T = 25˚C [V-C2] x = 0, 0 < y . 10–4, T = 660˚C [2005Sch] y = 0, 0 < x ≤ 7·10–5, T = 641˚C [1990Kas]
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
7
8
10
Al–Mo–U
. Table 2 (continued) Phase/ Temperature Range [˚C] (Mo) < 2623
Pearson Symbol/ Lattice Space Group/ Parameters Prototype [pm] cI2 Im 3m W
a = 314.70
cI2 Im 3m W
a = 352.4
γ, U1–x–yMoxAly
a = 344.0
a = 343.9 β, (βU) (h1) 776 - 668 β, U1–x–yMoxAly
α, (αU) (r) < 668 α, U1–x–yMoxAly
λ2, U(MoxAl1–x)2
tP30 P42/mnm βU
a = 1075.9 c = 565.6
oC4 Cmcm αU
a = 285.37 b = 586.95 c = 495.48
cF24 Fd 3m Cu2Mg
UAl2 < 1620
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
T = 25˚C [V-C2]
x = 0, 0 < y ≤ 0.195, T = 2150˚C [2005Sch] y = 0, 0 < x ≤ 0.04, T ≈ 1800˚C [Mas2]
UxMo1–x–yAly
γ, (γU) (h2) 1135 - 776
Comments/References
T > 776˚C [V-C2]
x = 0, 0 < y ≤ 0.047,T = 1105˚C [1990Kas] y = 0, 0 < x ≤ 0.42, T = 1284˚C [Mas2] in the U95.2Mo2.8Al2.0 and U93.9Mo2.1Al4.0 (at.%) alloys annealed at 900˚C 48 h and cooled to room temperature at 4–5˚C·min–1, together with α and λ2 phases [1964Nic] in the U87.5Mo12.0Al0.5 (at.%) alloy homogenized at 1050˚C, reduced and quenched from 800˚C [1984Gom] T > 668˚C [V-C2]
x = 0, 0 < y ≤ 0.0054, T = 758˚C [1990Kas] y = 0, 0 < x ≤ 0.02, T = 668˚C [Mas2] T = 25˚C [V-C2]
x = 0, 0 < y < 7·10–4, T = 665˚C [1990Kas] y = 0, 0 < x ≤ 0.02, T = 570˚C [Mas2] 0 ≤ x ≤ 0.27 [1971Pet]
a = 778
[V-C2]
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Table 2 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Lattice Space Group/ Parameters Prototype [pm]
Comments/References
UAl3 < 1350
cP4 Pm3m AuCu3
a = 426.2
UAl4 < 731
oI20 Imma UAl4
a = 440.14 [2004Tou] b = 625.52 c = 1372.79
Mo3Al ≲ 2150
cP8 Pm3m Cr3Si
ξ2, MoAl 1750 - 1470
[V-C2]
a = 495
23 to 28.5 at.% Al at T ≈ 1720˚C [2005Sch] [1958Woo, 2005Sch]
a = 309.8
46 at.% Al at T ≈ 1720˚C to 52 at.% Al at T = 1570˚C [2005Sch] [1971Rex, 2005Sch]
cP2 Pm3m CsCl
ξ1, Mo2Al3 1570 - 1490
-
-
63 at.% Al [2005Sch]
Mo3Al8 < 1555
mC22 C2/m Mo3Al8
a = 916.4 b = 363.9 c = 1004 β = 100.5˚
[V-C2]
MoAl3 1222 - 818
mC32 C2/m MoAl3
a = 1639.6 [2005Sch] b = 359.4 c = 838.6 β = 101.88˚
Mo1–xAl3+x 1260 - 1154
cP8 Pm3m Cr3Si
76 at.% Al at T = 1222˚C to 78 at.% Al at T = 1154˚C [2005Sch] a = 494.5
[2005Sch]
MoAl4 1177 - 942
mC30 Cm WAl4
Mo4Al17 < 1034
mC84 C2 Mo4Al17
a = 915.8 b = 493.23 c = 2893.5 β = 96.71˚
[1995Gri, 2005Sch]
Mo5Al22 964 - 831
oF216 Fdd2 Mo5Al22
a = 7382 b = 916.1 c = 493.2
[1995Gri, 2005Sch]
Landolt‐Bo¨rnstein New Series IV/11E1
79 to 80 at.% Al at T = 1154˚C [2005Sch] a = 525.5 [V-C2] b = 1776.8 c = 522.5 β = 100.88˚
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
9
10
10
Al–Mo–U
. Table 2 (continued) Phase/ Temperature Range [˚C]
Pearson Symbol/ Lattice Space Group/ Parameters Prototype [pm]
MoAl5 (h2) 750 - 800 < T < 846
hP12 P6322 WAl5
a = 491.2 c = 886.0 a = 493.7 c = 924.3
[2005Sch]
MoAl5 (h1) 648 < T < 750–800
hP60 P321
a = 493.3 c = 4398
[2005Sch]
Comments/References
Space group [P63V-C2]
MoAl5 (h1) MoAl5 (r) ≲ 648
hP36 R3c MoAl5 (r)
a = 495.1 c = 2623
[2005Sch]
MoAl12 < 712
cI26 Im3 WAl12
a = 757.3
[1954Ada, 2005Sch]
U2Mo ≲ 1252 (?)
tI6 I4/mmm MoSi2
a = 342.7 c = 983.4
* τ1, U9Mo16Al75
-
-
[1969Pet]
-
0.31 ≤ x ≤ 0.40 [1969Pet]
* τ2, U(MoxAl1–x)2 hP12 P63/mmc MgZn2
32.5 to 34 at.% Mo [Mas2] [V-C2]
* τ3, U6Mo4Al43
hP2 a = 1096.6 P63/mcm c = 1769.0 Ho6Mo4+xAl43–x (x = 0.11) or Yb6Cr4+xAl43–x (x = 1.15)
[1994Nie]
* τ4, UMo2Al20
cF8 Fd3m CeTi2Al20 or CeCr2Al20
[1995Nie]
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
a = 1450.6
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
10
Al–Mo–U
. Table 3 Invariant Equilibria Composition (at.%) Reaction
T [˚C]
Type
Phase
L + ξ1 Ð Mo3Al8 + ξ2
1510
U1
L
L + ξ2 Ð Mo3Al8 + Mo3Al
L + λ2 Ð τ2
L Ð τ2 + Mo3Al
1480
1460
1410
U2
p3
e5
1380
U3
ξ1
63.0
37.0
0
Mo3Al8
72.7
27.3
0
ξ2
48.0
52.0
0
60.0
30.0
ξ2
48.0
52.0
0
Mo3Al8
72.7
27.3
0
Mo3Al
25.0
75.0
0
L
45.2
21.5
33.3
L
L Ð λ2 + Mo3Al8 + Mo3Al
1340
U4
E1
1220
U5
48.2
18.5
33.3
46.0
20.7
33.3
L
39.0
29.0
32.0
τ2
39.7
27.0
33.3
25.0
75.0
L
48.5
27.5
24.0
τ2
45.5
21.5
33.3
MSIT1
0
49.0
18.0
25.0
75.0
66.4
18.3
15.3
τ1
75.0
16.0
9.0
λ2
61.0
6.0
33.0
Mo3Al8
72.7
27.3
0
L
58.0
26.0
16.0
58.5
8.5
33.0
Mo3Al8
72.7
27.3
0
Mo3Al
25.0
75.0
0
L
6.0
28.0
66.0
(Mo)
1.5
97.0
1.5
γ
1.0
39.0
60.0
25.0
75.0
L
Mo3Al
Landolt‐Bo¨rnstein New Series IV/11E1
10.0
λ2
λ2
L + (Mo) Ð γ + Mo3Al
4.0
τ2
Mo3Al 1352
U
29.5
λ2 L + τ1 Ð Ð λ2 + Mo3Al8
Mo 66.5
Mo3Al L + τ2 Ð λ2 + Mo3Al
Al
33.3 0
0
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
11
12
10
Al–Mo–U
. Table 3 (continued) Composition (at.%) Reaction
T [˚C]
Type
Phase
L + Mo3Al Ð γ + τ2
1140
U6
L
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
1115
U7
MSIT1
Mo
U
9.0
22.0
25.0
75.0
γ
3.0
24.0
73.0
τ2
39.2
27.0
33.8
L
11.5
10.5
78.0
Mo3Al
L + τ2 Ð γ + λ 2
Al
69.0 0
τ2
44.8
21.5
33.7
γ
4.5
11.5
84.0
λ2
50.4
15.8
33.8
Landolt‐Bo¨rnstein New Series IV/11E1
10
. Fig. 1a Al-Mo-U. Partial reaction scheme, part 1
Al–Mo–U
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
13
10
Al–Mo–U
. Fig. 1b Al-Mo-U. Partial reaction scheme, part 2
14
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Fig. 2 Al-Mo-U. Partial liquidus surface projection
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
15
16
10
Al–Mo–U
. Fig. 3 Al-Mo-U. Partial isothermal section at 1250˚C (U-UAl2-Mo3Al8-Mo region)
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Fig. 4 Al-Mo-U. Partial isothermal section at 1050˚C (U-UAl2-Mo3Al8-Mo region)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
17
18
10
Al–Mo–U
. Fig. 5 Al-Mo-U. Partial isothermal section at 500˚C (U-UAl2-Mo3Al8-Mo region)
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Fig. 6 Al-Mo-U. Temperature - composition section UAl2-Mo3Al8
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
19
20
10
Al–Mo–U
. Fig. 7 Al-Mo-U. Isopleth at 33.3 at.% U
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Fig. 8 Al-Mo-U. Temperature - composition section U52Al48-Mo3Al (plotted in at.%)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
21
22
10
Al–Mo–U
. Fig. 9 Al-Mo-U. Isopleth at 40 at.% Mo
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Fig. 10 Al-Mo-U. Isopleth at 20 at.% Al
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
23
24
10
Al–Mo–U
. Fig. 11 Al-Mo-U. Isopleth at 50 at.% Al
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
. Fig. 12 Al-Mo-U. Isopleth at 20 at.% Mo
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
25
26
10
Al–Mo–U
. Fig. 13 Al-Mo-U. Isopleth at 80 at.% U
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Mo–U
10
References [1954Ada] [1958Woo]
[1964Nic]
[1969Pet] [1971Pet] [1971Rex]
[1979Sof]
[1980Fer] [1984Gom]
[1990Kas]
[1993Ale]
[1994Nie] [1995Gri] [1995Nie]
[1997Lee]
[2000Han]
[2002Kim]
[2002Lee]
[2002Mey]
Adam, J., Rich, J.B., “The Crystal Structure of WAl12, MoAl12 and (Mn, Cr)Al12”, Acta Cryst., (7), 813–816 (1954) (Crys. Structure, Experimental, 14) as quoted by [2005Sch] Wood, E.A., Compton, V.B., Matthias, B.T., Corenzwit, E., “β-Wolfram Structure of Compounds Between Transition Elements, Gallium and Antimony”, Acta Crystallogr., (11), 604–606 (1958) (Crys. Structure, Experimental, 13) as quoted by [2005Sch] Nicholson, S., Harris, D.G., Stobo, J.J., “The Effect of Ternary Additions on the Microstructures of Dilute U-Mo Alloys”, J. Nucl. Mater., 12(2), 173–183 (1964) (Crys. Structure, Morphology, Phase Relations, Experimental, 13) Petzow, G., Rexer, J., “Liquid Equilibria in the Uranium-UAl2-Al8Mo3-Mo System” (in German), Z. Metallkd., 60(5), 449–453 (1969) (Morphology, Phase Diagram, Phase Relations, Experimental, #, 14) Petzow, G., Rexer, J., “Phase Equilibria in the Uranium-UAl2-Al8Mo3-Mo System” (in German), Z. Metallkd., 62(1), 34–38 (1971) (Phase Diagram, Phase Relations, Experimental, #, 9) Rexer, J., “Phase Equilibria in the System Al-Mo at Temperatures above 1400˚C” (in German), Z. Metallkd., 62, 844–848 (1971) (Crys. Structure, Phase Diagram, Experimental, 23) as quoted by [2005Sch] Sofronova, R.M., Nikolaev, A.G., Lyutina, E.M., Voytekhova, E.A., “Influence of Al, Mn, Pd, Ir and Pt Additions on Martensitic Transformation γ → α’b in Uranium Alloys” (in Russian), Alloys for Atomic Energy, Ivanov, O.S., Alekseeva, Z.M. (Eds.), Nauka, Moscow, 131–134 (1979) (Crys. Structure, Morphology, Phase Relations, Experimental, 7) Ferro, R., Marazza, R., “Crystal Structure and Density Data”, Atomic Energy Rev.: Spec. Iss., (7), 359–507 (1980) (Crys. Structure, Phase Relations, Review, 961) Gomozov, L.I., Pokrovskii, A.A., “Influence of Additional Alloying on α-Phase Transformation Kinetics in a Uranium Alloy with 12 at.% Molybdenum”, Russ. Metall. (Engl. Transl.), (4), 142–146 (1984), translated from Izv. Akad. Nauk SSSR, Met., (4), 136–140 (1984) (Crys. Structure, Morphology, Phase Relations, Experimental, Kinetics, Mechan. Prop., 11) Kassner, M.E., Adamson, M.G., Adler, P.H., Peterson, D.E., “The Al-U (Aluminium-Uranium) System”, Bull. Alloy Phase Diagrams, 11(1), 82–89 (1990) (Crys. Structure, Phase Diagram, Thermodyn., Assessment, 44) Alekseeva, Z.M., “Aluminium - Molybdenum - Uranium”, MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.22243.1.20, (1993) (Crys. Structure, Phase Diagram, Assessment, #, 6) Niemann, S., Jeitschko, W., “Ternary Aluminides A6T4Al43 with A = Y, Nd, Sm, Gd-Lu, Th, U and T = Cr, Mo, W”, Z. Metallkd., 85(5), 345–349 (1994) (Crys. Structure, Experimental, 23) Grin, Y.N., Ellner, M., Peters, K., Schuster, J.C., “The Crystal Structure of Mo4Al17 and Mo5Al22”, Z. Krist., 210, 96–99 (1995) (Crys. Structure, Experimental, 11) as quoted by [2005Sch] Niemann, S., Jeitschko, W., “Ternary Aluminides AT2Al20 (A = Rare Earth Elements and Uranium; T = Ti, Nb, Ta, Mo, and W) with CeCr2Al20-Type Structure”, J. Solid State Chem., 114, 337–341 (1995) (Crys. Structure, Experimental, 18) Lee, D.B., Kim, K.H., Kim, C.K., “Thermal Compatibility Studies of Unirradiated U-Mo Alloys Dispersed in Aluminium, J. Nucl. Mater., 250(1), 79–82 (1997) (Morphology, Experimental, Interface Phenomena) cited from abstract Han, Y.-S., Park, J.-M., Kim, K.-H., Lee, Y.-S., Kim., C.-K., “An Investigation on the Green Properties of U-10 wt% Mo/Al and U3Si2/Al Powder Compacts”, Nucl. Eng. Design, 202(1), 1–9 (2000) (Morphology, Experimental, Mechan. Prop., 24) cited from abstract Kim, K.H., Park, J.M., Kim, C.K., Hofman, G.L., Meyer, M.K., “Irradiation Behavior of Atomized U-10 wt.% Mo Alloy Aluminum Matrix Dispersion Fuel Meat at Low Temperature”, Nucl. Eng. Design, 211 (2-3), 229–235 (2002) (Morphology, Experimental, Kinetics) cited from abstract Lee, J.-S., Lee, Ch.-H., Kim, K.H., Em, V., “Study of Decomposition and Reactions with Aluminum Matrix of Dispersed Atomized U-10 wt% Mo Alloy”, J. Nucl. Mater., 306(2-3), 147–152 (2002) (Crys. Structure, Morphology, Phase Relations, Experimental, Kinetics, 6) Meyer, M.K., Hofman, G.L., Hayes, S.L., Clark, C.R., Wiencek, T.C., Snelgrove, J.L., Strain, R.V., Kim, K.H., “Low-Temperature Irradiation Behavior of Uranium-Molybdenum Alloy Dispersion Fuel, J. Nucl. Mater., 304(2-3), 221–236 (2002) (Morphology, Experimental, Kinetics) cited from abstract
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
27
28
10 [2003Gar]
[2003Lee]
[2003Mir]
[2003Ryu]
[2004Kei]
[2004Lee]
[2004Tou] [2005Sch]
[2006Kim]
[2006Ryu1] [2006Ryu2]
[2006Wie]
[2007Noe]
[2007Sob]
[Mas2] [V-C2]
Al–Mo–U Garces, J.E., Marino, A.C., Bozzolo, G., “Theoretical Description of the Interdiffusion of Al in the U-Mo Solid Solution”, Appl. Surf. Sci., 219, 47–55 (2003) (Morphology, Calculation, Theory, Interface Phenomena, 11) Lee, S.H., Kim, J.C., Park, J.M., Kim, C.K., Kim, S.W., “Effect of Heat Treatment on Thermal Conductivity of U-Mo/Al Alloy Dispersion Fuel”, Intern. J. Thermophys., 24(5 Special Issue SI), 1355–1371 (2003) (Morphology, Calculation, Experimental, Phys. Prop., 10) cited from abstract Mirandou, M.I., Balart, S.N., Ortiz, M., Granovsky, M.S., “Characterization of the Reaction Layer in U-7 wt% Mo/Al Diffusion Couples”, J. Nucl. Mater., 323(1), 29–35 (2003) (Crys. Structure, Morphology, Phase Relations, Experimental, Interface Phenomena, Kinetics, Transport Phenomena, 18) Ryu, H.J., Han, Y.S., Park, J.M., Park, S.D., Kim, C.K., “Reaction Layer Growth and Reaction Heat of U-Mo/Al Dispersion Fuels Using Centrifugally Atomized Powders”, J. Nucl. Mater., 321, 210–220 (2003) (Crys. Structure, Morphology, Phase Relations, Thermodyn., Experimental, Interface Phenomena, Kinetics, 31) Keiser, D.D., Jr., Clark, C.R., Meyer, M.K., “Phase Development in Al-Rich U-Mo-Al Alloys”, Scr. Mater., 51, 893–898 (2004) (Crys Structure, Morphology, Phase Relations, Experimental, Interface Phenomena, 11) Leenaers, A., Van den Berghe, S., Koonen, E., Jarousse, C., Huet, F., Trotabas, M., Boyard, M., Guillot, S., Sannen, L., Verwerft, M., “Post-irradiation Examination of Uranium-7 wt% Molybdenum Atomized Dispersion Fuel”, J. Nucl. Mater., 335 (1), 39–47 (2004) (Crys. Structure, Morphology, Phase Relations, Experimental, Interface Phenomena, 18) Tougait, O., Noel, H., “Stoichiometry of UAl4”, Intermetallics, 12, 219–223 (2004) (Crys. Structure, Experimental, 24) Schuster, J.C., “Al-Mo (Aluminium-Molybdenum)”, MSIT Binary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services, GmbH, Stuttgart; Document ID: 30.12123.1.20, (2005) (Crys. Structure, Phase Diagram, Assessment, 61) Kim, Y.S., Hofman, G.L., Ryu, H.J., Hayes, S.L., “Irradiation-Enhanced Interdiffusion in the Diffusion Zone of U-Mo Dispersion Fuel in Al”, J. Phase Equilib. Diffus., 27(6), 614–621 (2006) (Morphology, Thermodyn., Calculation, Experimental, Interface Phenomena, Kinetics, 16) Ryu, H.J., Kim, Y.S., Hofman, G.L., Park, J.M., Kim, C.K., “Heats of Formation of (U,Mo)Al3 and U(Al, Si)3”, J. Nucl. Mater., 358, 52–56 (2006) (Morphology, Thermodyn., Experimental, 10) Ryu, H.J., Park, J.M., Kim, C.K., Kim, Y.S., Hofman, G.L., “Diffusion Reaction Behaviors of U-Mo/Al Dispersion Fuel”, J. Phase Equilib. Diffus., 27(6), 651–658 (2006) (Crys. Structure, Morphology, Phase Relations, Experimental, Interface Phenomena, Kinetics, 21) Wieschalla, N., Bergmaier, A., Boeni, P., Boening, K., Dollinger, G., Grossmann, R., Petry, W., Roehrmoser, A., Schneider, J., “Heavy Ion Irradiation of U-Mo/Al Dispersion Fuel”, J. Nucl. Mater., 357, 191–197 (2006) (Morphology, Phase Relations, Experimental, Interface Phenomena, 9) Noel, H., Tougait, O., Potel, M., “Crystal Structures and Phase Stoichiometry of Nuclear Materials in the U-Si-C and U-Mo-Al Systems”, Collected Abstracts of the X International Conference on Crystal Chemistry of Intermetallic Compounds, Lviv, Ukraine, 17–20 September, 2007, Ivan Franko National University of Lviv, 5 (2007) (Crys. Structure, Experimental, 4) Soba, A., Denis, A., “An Interdiffusional Model for Prediction of the Interaction Layer Growth in the System Uranium-Molybdenum/Aluminum”, J. Nucl. Mater., 360, 231–241 (2007) (Morphology, Calculation, Theory, Interface Phenomena, Kinetics, 22) Massalski, T.B. (Ed.), Binary Alloy Phase Diagrams, 2nd edition, ASM International, Metals Park, Ohio (1990) Villars, P. and Calvert, L.D., Pearson’s Handbook of Crystallographic Data for Intermetallic Phases, 2nd edition, ASM, Metals Park, Ohio (1991)
DOI: 10.1007/978-3-540-88053-0_10 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
Aluminium – Niobium – Nickel Refractory Metal Systems: Phase Diagrams, Crystallographic and Thermodynamic Data Lesley Cornish, Damian M. Cupid, Joachim Gro¨bner, Annelies Malfliet
Introduction Knowledge of the phase equilibria and thermodynamic properties of the Al-Nb-Ni system is relevant for many applications, especially for nickel-based superalloys. Pertinent to this is the order-disorder transformation between the disordered (Ni) and the ordered L12-Ni3Al [2003Du]. The excellent high temperature strength and high corrosion resistance of the binary intermetallic compound Ni3Al can be improved by alloying Nb to this compound, and this element has a large ternary solubility [2003Cer1]. The first experimental work on the Al-Nb-Ni system was by [1962Min1, 1962Min2] and [1965Kor], who both constructed the quasibinary section between Ni3Al and NbNi3. [1966Mar] determined the isothermal sections of most of the phase diagram at 900 and 1140˚C. Other investigations are mostly concentrated on the Ni rich corner [1970Cis, 1970Duv, 1979Oma, 1983Och, 1969Gus, 1989Hon]. The phase relations and homogeneity range of Ni3Al are studied by [1980Nas, 1994Jia]. An evaluation of the ternary Al-Nb-Ni system is made by [1993Sau]. [1992Lee, 2003Du, 2006Rag] reviewed the literature published up to this date. A Calphad type calculation of the entire phase diagram is reported by [2003Du], which is in good agreement with most of the experimental data. Although this calculation did not agree with all the experimental data, it has the best overall fit for describing the whole system. In cases where the agreement was less good, this was deduced to be because the samples had been annealed for relatively short times, considering the high melting points of most of the phases. Typically, at least 1200 h would be a reasonable annealing time for high temperature phases in bulk alloys with high melting compounds. Additionally, in all the isothermal sections calculated by [2003Du], the NbNi3 phase had an improbable shape in that there was some extension into the ternary on the Ni rich side, but not on the Nb rich side, and this has been smoothed in the present evaluation. An overview of the investigations considering phase equilibria, solid phases and thermodynamics of the system is given in Table 1.
Binary Systems The phase diagram of the binary Nb-Ni system is adopted from the calculations of [2006Che], which is in good agreement with most available experimental data. It is an extension of [2003Du], but used more recent experimental data. This diagram is redrawn in Fig. 1, but to be consistent with the other binary and ternary data the melting point of Nb is lowered from 2477 to 2469˚C. The binary Al-Ni phase diagram is taken from the MSIT evaluation by
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
1
2
11
Al–Nb–Ni
[2004Sal]. For the Al-Nb phase diagram, [Mas2] was accepted, with additional information on the Al rich liquidus Al-Nb was taken from [1973Wil].
Solid Phases The binary and ternary phases of the Al-Nb-Ni system are listed in Table 2. [1966Ben, 1968Hun] reported that the NbNi phase takes up a considerable quantity of Al. The binary phases, NbNi and Ni3Al have considerable extension into the ternary system [1966Ben]. [1968Hun] confirmed the large solubility of Al in the NbNi phase to be about 35 at.% Al. [1969Gus] measured a solubility of about 10 at.% Nb in Ni3Al, which only varied slightly over the temperature range 800 - 1200˚C. [1980Nas] confirmed this solubility at 1200˚C. The variation of the lattice parameter of Ni3Al along the line Ni3Al - NbNi3 was quite well established by [1962Min1, 1963Arb, 1969Gus, 1970Cis, 1980Nas, 1984Och1]. [1980Nas] reported a solubility of at least 5.5 at.% Nb in NiAl in equilibrium with τ1 and NbNi3 at 1200˚C. There are at least three true ternary phases τ1, τ2 and τ3 (denoted as H, L and M in the original literature) which exist only in the ternary diagram. The first data on these phases arose from [1964Sch, 1965Mar, 1965Ram]. They basically agree on the existence of the τ1, NbNi2Al, a Heusler type phase and τ2, Nb(Al,Ni)2 with a MgZn2 type structure. [1965Ram] reported that a phase, isostructural with Ti2Ni, exists in equilibrium with the τ1 phase, but no other studies report this phase. The τ2 phase has extensive solubility of Ni and Al confirming the formula Nb(AlxNi1–x)2, where x varies from 0.19 to 0.83 [1966Ben]. This result agrees with the data of [1966Mar]. In addition, above 900˚C an orthorhombic phase τ3 structurally related to the NbNi phase forms [1966Ben, 1967Sho, 1968Hun]. According to the phase diagram of [1966Ben], the τ3 phase extends from about 3 to 30 at.% Al. However, [1968Hun] observed a smaller homogeneity range for the τ3 phase. In addition, he found an additional ternary phase with higher Al content and like τ3, with a structure similar to NbNi. The discrepancy between the two authors could result from the difference in annealing time as [1966Ben] annealed only 20 h, while [1968Hun] used 168 h. However, [1968Hun] used only a limited number of samples, and the phase relations in his isothermal section are unusual. As no other experimental investigations report on this phase region, this part of the phase diagram is questionable. [1966Mar] did not observe the ternary τ3 phase at 900˚C and only a small extension of NbNi into the ternary. Thermal conductivity contours were used to determine the site preference of Nb in Ni3Al [2001Ter], and ab-initio calculations were used to investigate the site preference of Nb substitution in NiAl [2000Boz, 2001Son, 2002Boz]. Calculations based on the d-orbital level of the transition metals [1985Mor] as well as ab-initio methods [1991Eno] were used to predict the phase boundaries between NiAl and Ni3Al with dissolved Nb. First principles calculations were also used to calculate the relative stability of L12-Cu3Au and D0a-βCu3Ti structures of Ni3Al and NbNi3, each with additional Nb and Al respectively [1996Rav]. [2001Sav] used electrical resistivity measurements to examine the long range ordering of Ni3Al with Nb additions as a function of temperature. Order-disorder transition temperatures and the kinetics of the transition were studied [2001Sav].
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
Quasibinary Systems [1965Kor] established that a simple quasibinary eutectic exists between NiAl and τ2 with stoichiometry NbNiAl, with the eutectic temperature and composition being respectively 1437˚C and 16.5 at.% Nb (Fig. 2). However, it should be noted that the thermal analysis data reported in tabular form give a 40˚C temperature range for the eutectic which would be very close to the maximal experimental error at that time. Thus, it is not fully conclusive with these data that the section is a true quasibinary. The position of the eutectic point does not coincide with that of the calculation of [2003Du], and in Fig. 6, the surface of solidification for τ2 has been moved to accommodate the experimental data. In addition, the solubility of Nb in the NiAl phase is less than might be expected from the measurements for NiAl in equilibrium with the τ1 phase [1980Nas], although the two measurements were from slightly different NiAl compositions.
Invariant Equilibria A ternary eutectic reaction (L Ð (Ni) + NiAl3 + NbNi3) was identified by [1973Kra] and [1973Lem] at 1270˚C and 13.6 at.% Nb and 79.1 at.% Ni. From this and the work of [1962Min1, 1962Min2, 1965Kor, 1969Nov] invariant reactions involving the liquid were deduced by [1992Lee]. [1992Lee] also included a possible ternary transition type solid state reaction NiAl + NbNi3 Ð NiAl3 + τ1. However, the evidence for this is considered too speculative here, and the reaction has not been included in Fig. 3, which is from the calculation of [2003Du]. [2003Rio] reported an invariant reaction L Ð NbAl3 + Nb2Al + τ2 at 1553˚C by DTA, with the ternary eutectic composition very near to the binary eutectic L Ð NbAl3 + Nb2Al. This is 150˚C higher than calculated by [2003Du], and the micrographs of [2003Rio] convincingly show three eutectic phases. Therefore, the calculated temperature is taken to be less reliable. The compositions of the phases participating in the invariant reactions are listed in Tables 3 and 4 as digitized from Fig. 4.
Liquidus, Solidus and Solvus Surfaces The liquidus of Ni rich alloys was determined by [1969Nov, 1973Kra, 1973Lem]. Based on these studies [1969Nov, 1973Kra, 1973Lem], [2003Du] undertook thermodynamic calculations and constructed a liquidus projection, which is shown in Fig. 4 [2003Du]. [2001Miu] investigated liquidus and solidus lines in the Ni rich corner between 1325 and 1450˚C (Figs. 5 and 6), which are consistent with the calculated results of [2003Du]. Both Fig. 5 and Fig. 6 are not adjusted to the accepted binary diagrams. The solvus line of (Ni) was reported by [1989Hon] and [2001Miu]. The solvus line of (Ni) [2001Miu] is shown in Fig. 7, and is qualitatively in agreement with [1989Hon].
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
3
4
11
Al–Nb–Ni
Isothermal Sections There have been a number of detailed studies of solid state equilibria in the Ni-rich region of the phase diagram: at 1300˚C by [1994Jia], at 1200˚C by [1962Min1, 1962Min2, 1970Cis, 1970Duv, 1980Nas, 1975Bok, 1994Jia, 1997Uey], at 1100˚C [1994Jia], at 1080˚C by [1975Bok], at 1000˚C by [1970Cis, 1983Och] at 800˚C by [1970Cis, 1969Gus, 1975Bok, 1994Jia], at 750˚C by [1970Duv] and at 600˚C by [1979Oma]. [1962Min1, 1962Min2, 1970Cis, 1970Duv, 1983Och] used both X-ray diffraction and metallography, while [1969Gus] used X-ray diffraction. A study by [1980Nas] used a variety of techniques which included metallography, X-ray diffraction and electron microprobe analysis. [1966Mar] using X-ray diffraction and [1966Ben] using both X-ray diffraction and metallography determined isothermal sections of almost the complete phase diagram at 900 and 1140˚C, respectively. In all the calculated sections, the NbNi3 phase showed some extension on the Ni rich side but not on the Nb rich side, and all of these have been smoothed here. The isothermal section at 1300˚C is given in Fig. 8. It is taken from the calculation by [2003Du] and in good agreement with the tie lines between (Ni) and Ni3Al measured by [1994Jia], although the agreement between NiAl3 and NiAl is less good, but acceptable. At 1200˚C (Fig. 9), [1962Min1, 1962Min2, 1970Cis, 1970Duv, 1975Bok, 1980Nas, 1994Jia, 1997Uey] show good agreement with [2003Du], although the (Ni) boundaries of [1970Cis] were slightly reduced, but within experimental error, especially considering that the samples have been annealed for only 65 h. [1980Nas] agrees with [2003Du], except for the minor phase analyses of two alloys which were probably compromised by the major phase (since the alloy composition was nearer to that of the major phase). In [1966Ben], the isothermal section at 1140˚C shows a three-phase field between τ2, NbAl3 and NiAl. This section is characterized by extensive solubility of the Ni3Al and NbNi phases in the ternary and the existence of three ternary compounds τ1, τ2 and τ3. In the calculated section [2003Du] (Fig. 10), the data point of NbAl3 [1966Ben] falls in a different phase field. However, this could be explained by the retention of NbAl3 due to a short annealing time (20 h), and so does not compromise the isothermal section of [2003Du]. At 1080˚C, the calculated isothermal section of [2003Du] (Fig. 11) is in good agreement with the experimental isothermal section of [1994Jia]. For the 1027˚C isothermal section, as shown in Fig. 12, the experimental data of [1983Och] show very good agreement with [2003Du], although Ni3Al boundary has a slight discrepancy. However, the experimental results of [1989Hon] for the three-phase region (Ni) + NbNi3 + Ni3Al do not fall in the calculated three-phase region of [2003Du], this could be because the alloys were only annealed for 555 h. The isothermal section at 900˚C of [2003Du] is given in Fig. 13. Most of the data at 900˚C [1966Mar] agree with [2003Du], except for the extension for NbNi for which [1966Mar] shows a very limited extent. The greater extent of NbNi might not have been observed due to the lack of equilibrium after annealing the alloys for only the relatively short time of 700 h (Nb having a high melting point would be slow to diffuse), and the high temperature Nb2Al phase might not have disappeared in this time. The extent of NbNi would fall in the NbNi-Nb2Al two-phase field of [1966Mar], and the identified three-phase fields could be due to a third phase which is still disappearing on annealing. Only partial isothermal sections were calculated at 800˚C, and these are shown in Figs. 14a and 14b. In the Ni rich corner at 800˚C (Fig. 14a), the experimental results for the position of the two-phase (Ni) + Ni3Al region [1969Gus, 1970Cis, 1994Jia] are not in agreement with the DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
calculation of [2003Du], but they were not used for the optimization. However, it must be pointed out that these three sets of experimental data agree well with each other, suggesting that the (Ni) actually has a lower solubility at 800˚C than is accepted by [2003Du]. Additionally, [1969Gus] shows that the (Ni) + Ni3Al two-phase field penetrates further into the ternary than that calculated by [2003Du]. The isothermal section at 800˚C in Fig. 14a was redrawn ensuring the NbNi3 phase is consistent with the accepted binary diagram. The Al rich corner at 800˚C (Fig. 14b) was investigated experimentally by [1965Mar] and the results are in fairly good agreement with the calculated work of [2003Du], even though they were not included in the optimization [2003Du]. Figure 15 shows the isothermal section at 750˚C. The experimental results of [1970Duv] in the Ni rich corner are in good agreement with each other, although (Ni) shows less solubility of Al and more for Nb than calculated by [2003Du]. Similarly, the isothermal section at 600˚C (given in Fig. 16) has some discrepancy between the experimental [1979Oma] and calculated results [2003Du], with the position of the two-phase Ni2Al3+NbAl3 region being slightly different. In general, the studies of [1962Min1, 1962Min2, 1969Gus, 1970Duv, 1980Nas, 1983Och] agree to within ±2 at.% Al and 1 at.% Nb on the composition of the three-phase equilibrium (Ni), Ni3Al and NbNi3, except [1980Nas] who reported up to 2 at.% Al solubility in NbNi3, while the other studies suggest that the solubility is very small. The results of [1970Cis] are quite different from these studies and have not been accepted here.
Temperature – Composition Sections A temperature-composition section at a constant 2.5 mass% Al showing the (Ni), Ni3Al and NbNi3 phases was produced by [1975Bok] experimentally, but is not consistent with the ternary diagrams accepted here (that of [2003Du] with some modifications in the liquidus surface) because of the shape of the liquidus near (Ni). [1962Min1, 1962Min2, 1965Kor] examined liquid/solid as well as solid state equilibria in two separate isopleths. [1962Min1, 1962Min2] examined alloys formed between Ni3Al and NbNi3 using thermal analysis, metallography, X-ray diffraction, hardness and resistivity measurement and established that a eutectic reaction exists between Ni3Al and NbNi3 at 1280˚C and 16 at.% Nb. This temperature-composition section is not a completely true quasibinary, since Ni3Al does not melt congruently. The temperatures of [1962Min1, 1962Min2] are close, although not in exact agreement, to the accepted Al-Ni binary, but are acceptable within experimental limits of that time. The composition of Ni3Al at the eutectic temperature was also determined by [1963Arb], and later [1969Tho], using metallography, reported that the eutectic composition is slightly lower in Nb at 15.4 at.% Nb. [1963Arb] carefully determined the solubility of Nb in Ni3Al at the quasibinary eutectic temperature using diffraction methods. Both of these additional studies are taken into account in Fig. 17 which has also been slightly altered from [1962Min1, 1962Min2] to be consistent with the AlNi binary system accepted here [2004Sal]. The calculated temperature-composition Ni3Al NbNi3 by [2003Du] is in good agreement with the experimental data of [1962Min1, 1963Arb, 1969Tho], except that the experimental results show less temperature dependence for Ni3Al.
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
5
6
11
Al–Nb–Ni
Thermodynamics A detailed thermodynamic modelling after the Calphad method was published by [2003Du]. Most of the available experimental information for the Al-Nb-Ni system was used for this calculation, except for those alluded to above [1965Mar, 1969Gus, 1970Cis, 1994Jia]. No fundamental discrepancies between the different experimental information taken from literature were observed. Experimental thermodynamic data were not available for this work. More recently [2006Hu] reported enthalpies of formation for two ternary phases τ1 and τ2 as well as other phases, and selected values are given in Table 5.
Notes on Materials Properties and Applications The most important application of the Al-Nb-Ni system is in the Ni-based superalloys, which can have up to 14 components. The matrix of this alloys comprised (Ni) and the major precipitates are based on Ni3Al. However, with increasing addition, the precipitates can be more complex. Nb is a useful addition for increasing the melting points. The Al-Nb-Ni system is also of interest as a metallic glass, with Al particles embedded in the glass phase, for structural materials. The glass formation and crystallization temperatures of amorphous (Ni60Nb40)100–xAlx alloys were investigated using differential scanning calorimetry [1987Akh, 2007Yu] and differential scanning calorimetry with differential thermal analysis [2004Lee]. [2007Yu] found that although the amorphous phase was resistant to attack by Al, the crystallized phase was not. Al87Ni10Nb3 was examined by [2004Aud], and He2+ ion bombardment [1991Ska], along with rapid quenching, and mechanical milling [2004Dia] were used to generate amorphous metal phases from NbNiAl and Nb45Ni50Al5 alloys. The Young’s modulus, yield strength, and ultimate tensile strength of an Al-particle reinforced Ni70Nb30 metallic glass was studied by [2006Yu]. [1998Far] produced NiAl matrix composites reinforced with Nb particles by reactive hot pressing of the elemental powders. Microhardness and compressive yield strength of the alloys were measured. [1995Net] used combustion synthesis (of elemental powders) to prepare selected Al-Nb-Ni alloys. [2000DeL] found that excess Al not participating in the aluminothermic reduction reaction for the formation of a Ni-65Nb (mass%) alloy dissolved into the NbNi phase, which is in agreement with the solubility of Al in NbNi. The effect on creep strength of tungsten and molybdenum layers applied to NiAl + Nb powders prior to pressing was studied by [2006Bel]. The ternary eutectic reactions in the Al-Nb-Ni system were used to produce directionally solidified (DS) eutectic alloys with in-situ, aligned composite microstructures without grain boundaries as potential candidate materials for replacement of Ni-based superalloys. After confirming the NbAl3-NbNiAl-Nb2Al ternary eutectic [2000Rio], the influence of growth rate on microstructure [2002Rio, 2004Rio, 2005Cos] and mechanical properties [2002Rio] were examined. [1992Rev] directionally solidified a NiAl-NbNiAl alloy near the eutectic maximum in the ternary. [1975Kra] directionally solidified an alloy near to the (Ni)-Ni3Al-NbNi3 eutectic, and high-temperature strengths of similarly solidified alloys in the same region were investigated by [1984Tor]. Dislocation structures and mechanical properties of a directionally solidified eutectic alloy with (Ni) / Ni3Al matrix with strengthening NbNi3 phase were investigated by [1978Sve]. DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
Investigations have been made on NiAl for potential shape memory effect [2002Kim], although the beneficial transformation was blocked by the transformation to Ni5Al3. However, Nb additions were found to facilitate the desired transformation. [1991Gra] investigated the oxidation behavior of two- and three-phase alloys in the Al-Nb-Ni system with thermogravimetric analysis. Oxidation of τ2 (NbNiAl) displayed quasilinear oxidation kinetics, whereas oxidation of ternary alloys of τ2 (NbNiAl) with additions of NiAl and (NiAl + Nb3Al) displayed parabolic oxidation rates. The corrosion behavior of Al-Nb-Ni alloys in mixed gas atmospheres of H2/H2O/H2S were generally parabolic, although linear behavior was also observed [1993He]. [1980Bhe] investigated the effect of different Al-Nb-Ni coating compositions on the oxidation of a selected Al-Nb-Ni alloy. Three types of oxidation behaviors were observed that depended on coating microstructure: formation of protective Al2O3 coatings, formation of non-protective Nb-oxide scales, and formation of non-protective NiO scales.
Miscellaneous Ni76Al22Nb22 and Ni3Al0.75Nb0.25 alloys were shown to obey an empirical relationship between bulk modulus B, molar volume V, and electron density η determined by [2004Li] as B = η2V. [2003Cer1] studied the effect of Nb concentration on interdiffusion coefficients in Ni3Al alloys with Nb using diffusion couples. Similarly, [2003Cer2] measured the interdiffusion coefficients of Nb and Al in the temperature interval 1173–1533 K with a Ni3Al + Ni-0.15Al0.075Nb couple to ascertain the effect of site preference on interdiffusion coefficients. The elastic modulus of a single crystal of composition Ni-0.19Al-0.06Nb was investigated using the velocity of elastic waves of frequencies 5.5, 15, and 50 MHz [2006Rin]. The coefficient of linear expansion was examined in several alloys based on the Ni3Al-NbNi3 composition line [1967Arb]. The results showed an inverse relationship between amount of NbNi3 and the linear expansion coefficient. The low-temperature (3.2 K-10.3 K) specific heat of NbNi2Al was determined using adiabatic calorimetry [1999Roc] and used to calculate the electronic specific heat, Debye temperature, and Einstein temperature. The experimental results were compared to theoretical calculations using the linear “muffin-tin” orbital-tight-binding (LMTO-TB) method. Other experimental work includes the microalloying Nb to NiAl [1991Sas], the characterization of the unstable growth interface with Widmansta¨tten-like precipitates between ternary Ni3Al and ternary NiAl [2001Kai], and Ni6NbAl metastable phase formation [1984Lia] through melt spinning and splat quenching experiments. The reversible hydrogen absorption properties at room temperature of NbNi and Nb10Ni9Al3 were also explored [2003Jou].
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
7
8
11
Al–Nb–Ni
. Table 1 Investigations of the Al-Nb-Ni Phase Relations, Structures and Thermodynamics Temperature/Composition/Phase Range Studied
Reference
Method/Experimental Technique
[1962Arb]
XRD
Ni3Al-NbNi3 alloys
[1962Min1, 1962Min2]
Microscopy, thermal analysis, hardness, XRD
Vertical section Ni3Al-Ni3Nb
[1963Arb]
XRD, thermal analysis
Ni3Al-NbNi3 alloys at 1300˚C
[1964Sch]
XRD
Three ternary phases NbNi2Al, NbNiAl, NbNiAl2
[1965Gol]
Microchemical analysis, XRD
Ni3Al-NbNi3
[1965Kor]
Microscopy, thermal analysis, hardness, XRD
Vertical section NiAl to 40 at.% Nb
[1965Mar]
XRD, microstructure investigations NbNi2Al, NbNiAl annealed at 800˚C
[1965Ram]
XRD
NbNi2Al at 800˚C
[1966Ben]
Metallography, XRD
NbNiAl at 1140˚C
[1966Mar]
XRD
Complete composition range at 800 and 900˚C
[1967Sho]
XRD
Nb48Ni39Al13
[1968Hun]
XRD
Nb2Al region at 1000˚C
[1969Gus]
XRD
800, 1080 and 1200˚C in Ni rich range
[1969Nov]
Thermal analysis
Liquidus surface of Ni-Ni3Al-NbNi3 system
[1969Tho]
Metallography, chemical analysis
Ni3Al-NbNi3 alloys
[1970Cis]
Metallography, XRD and EPMA
Nickel rich corner at 800, 1000 and 1200˚C
[1970Duv]
Spectroscopy, light metallography, Ni rich corner (> 75 at.% Ni) at 750 and XRD 1200˚C
[1971Min]
XRD, microstructural analysis
Ni-Ni3Al-NbNi3 from room temperature to liquidus temperature
[1972Duv]
Optical metallography, TEM
750˚C Ni rich corner
[1973Kra, 1975Kra]
Directional solidification study, metallography, DTA
Ni-NbNi3-Ni3Al subsystem
[1973Lem]
Metallography, thermal analysis, XRD
Liquidus, Ni rich corner
[1973Wil]
Electronic structure calculation
Ni3Al at 1000˚C
[1975Bok]
Electron microscopy, solidification Ni-Ni3Al-NbNi3 at 800, 1080 and 1200˚C study
[1975Kau]
Calphad calculation
Complete composition range
[1978Gul]
Thermal analysis
Ni rich corner
[1979Oma]
Metallography, XRD
Complete system
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Table 1 (continued) Reference
Method/Experimental Technique
Temperature/Composition/Phase Range Studied
[1980Nas]
XRD, EPMA
Ni rich corner at 1200˚C
[1983Och]
Metallography, XRD
Solubility in Ni3Al at 1000˚C
[1984Arg]
XRD
Selected phases
[1984Bre]
Metallography, optical microscopy, Ni-Ni3Al-Nb Ni3 at 800, 1000 and 1200˚C SEM
[1984Och1]
XRD
(Ni), Ni3Al lattice parameters
[1984Och2]
Miedema calculation
Bond energies for Ni3Al with Nb
[1985Mis]
XRD
Ni3Al
[1985Tro]
XRD
τ2, NbNiAl (Laves phase)
[1986Bla]
XRD, metallography
NbNi2 from 800 to 1200˚C
[1988Mor]
Solidification study, XRD
Ni3Al at 1000˚C
[1989Hon]
DTA, optical microscopy, SEM
Solvus of Ni between 827 and 1227˚C
[1989Sub]
DTA, SEM, EPMA, XRD
Nb Al3 at 1300˚C
[1991Eno]
Cluster variation calculation
Ni and Ni3Al compositions below 1000˚C
[1991Ino]
Band structure calculations
NbAl3 with Ni substitutions
[1991Mis]
Metallography, XRD
(Ni) solvus surface
[1992Rev]
Metallography, SEM, EPMA
Al-16.5Nb-41.75Ni microstructures
[1994Jia]
EPMA, SEM
Ni rich corner at 800 and 1300˚C
[1997Uey]
SEM, EPMA, XRD
NbNi3 at 1200˚C
[2001Miu]
DTA
Ni rich corner from 900 to 1450˚C
[2002Kri]
XRD, DSC
Al-10Nb-50Ni and Al-10Nb-62Ni from room temperature to 700˚C
[2003Du]
Calphad calculation
Complete composition range above 600˚C
[2003Rio]
SEM, WDS, STA
Alloys: Al: 57.3–54.4; Nb: 41.8–33.3; Ni:0.9–12.3 (at.%)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
9
10
11
Al–Nb–Ni
. Table 2 Crystallographic Data of Solid Phases
Phase/ Temperature Range [˚C]
Pearson Symbol/ Space Group/ Prototype
Lattice Parameters [pm]
Comments/References
(Al) < 660.452
cF4 Fm 3m Cu
a = 404.96
pure Al at 25˚C [V-C2]
(Nb) < 2469
cI2 Im 3m W
a = 330.04
pure Nb at 25˚C [Mas2]
(Ni) < 1455
cF4 Fm 3m Cu
a = 352.40
pure Ni at 25˚C [Mas2]
NbAl3 < 1680
tI8 I4/mnm TiAl3
a = 384.1 c = 860.9
[1980Jor]
Nb2Al < 1940
tP30 P42/mnm σCrFe
a = 994.4 c = 517.2
66.7 at.% Nb [1980Jor]
Nb3Al < 2060
cP8 Pm 3n Cr3Si
a = 518.0
75 at.% Nb [1980Jor]
NiAl3 < 856
oP16 Pnma Fe3C
a = 661.3 b = 736.7 c = 481.1
[2004Sal]
Ni2Al3 < 1138
hP5 P3m1 Ni2Al3
a = 402.8 c = 489.1
36.8 to 40.5 at.% Ni [2004Sal]
β, NiAl < 1651
cP2 Pm 3m CsCl
a = 287
42 to 69.2 at.% Ni [2004Sal]
Ni5Al3 < 723
oC16 Cmmm Pt5Ga3
a = 753 b = 661 c = 376
63 to 68 at.% Ni [2004Sal]
γ´, Ni3Al < 1372
cP4 Pm 3m AuCu3
a = 356.77 a = 358.9 a = 356.32
73 to 76 at.% Ni [2004Sal]
NbNi < 1290
hR39 R3m W6Fe7
a = 489.4 c = 2674.0 a = 499.3 c = 2710.0
50 at.% Ni, 0 at.% Al [1968Hun] 24 at.% Ni, 30 at.% Al [1968Hun]
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
11
Al–Nb–Ni
. Table 2 (continued) Pearson Symbol/ Space Group/ Prototype
Phase/ Temperature Range [˚C]
Lattice Parameters [pm]
Comments/References
δ, NbNi3 < 1399
oP8 Pmmn TiCu3
a = 509.65 b = 423.23 c = 453.92
[1997Uey]
NbNi8
-
-
-
* τ1, NbNi2Al
cF16 Fm 3m BiF3
a = 597.0
25 at.% Al, 25 at.% Nb [1966Ben] ("H" phase)
* τ2, NbNiAl
hP12 P63/mmc MgZn2
a = 487.0 to 505.0 for formula Nb(AlxNi1–x)2 where x = 0.19 to c = 793.0 to 837.0 0.83 [1966Ben] ("L" phase)
* τ3, Nb10Ni9Al3
oP52 Pnma Nb10Ni9Al3
a = 930.3 b = 1626.6 c = 493.3
13 at.% Al, 48 at.% Nb [1967Sho], ("M" phase)
Metastable NbNi8 < 515
-
-
-
. Table 3 Invariant Four-Phase Equilibria Composition (at.%) Reaction
T [˚C]
Type
Phase
Al
L + Nb3Al Ð NbNi + (Nb)
1634
U1
L
Nb
Ni
29.00
51.00
20.00
L + Nb3Al Ð Nb2Al + NbNi
1633
U2
L
31.06
49.97
18.97
L+NbNi Ð NbNiAl + Nb10Ni9Al3
1547
U3
L
27.82
42.09
30.09
L + NbNi Ð Nb2Al + NbNiAl
1488
U4
L
49.18
38.11
12.71
L Ð NbAl3 +Nb2Al +NbNiAl
1408
E1
L
55.66
34.87
9.47
L Ð NbNi3 + Ni3Al + (Ni)
1267
E2
L
7.86
14.07
78.07
L + NiAl Ð NbNiAl + Ni3Al
1206
U5
L
16.28
21.56
62.16
L + NbNi3 Ð NbNiAl + Ni3Al
1205
U5
L
15.94
21.63
62.43
L + NbNiAl Ð Nb10Ni9Al3 + NbNi3
1203
U7
L
1.04
38.88
60.08
Ni3Al + NbNiAl Ð NiAl + NbNi3
1200
U8
-
-
-
-
L + Nb10Ni9Al3 Ð NbNi + NbNi3
1191
U9
L
0.58
40.21
59.21
NbNiAl + NiAl Ð NbNi2Al + NbNi3
1174
U10
-
-
-
-
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
11
12
11
Al–Nb–Ni
. Table 3 (continued) Composition (at.%) Reaction
T [˚C]
Type
Phase
NiAl + NbNi3 ÐNbNi2Al + Ni3Al
1117
U11
-
L + NbNiAl Ð NiAl + NbAl3
1082
U12
L + NiAl Ð NbAl3 + Ni2Al3
1051
Nb10Ni9Al3 + NbNi3 Ð NbNiAl + NbNi Nb2Al + NbNi Ð NbNiAl + Nb3Al
Nb
Ni
-
-
-
L
63.62
11.59
24.79
U13
L
69.86
6.47
23.67
1019
U14
-
-
-
-
947
U15
-
-
-
-
L
-
-
-
-
-
-
L + Ni2Al3 Ð NbAl3 + NiAl3
849
U16
Nb3Al + NbNi Ð NbNiAl + (Nb)
797
U17
NbNi + (Nb) Ð NbNi2Al + NbNiAl
779
U18
NbNiAl + (Nb) Ð NbNi2Al + Nb3Al
728
U19
L + NbAl3 Ð NiAl3 + (Al)
647
U20
Al
-
L
. Table 4 Invariant Three-Phase Equilibria Composition (at.%) Reaction
T [˚C]
Type
Phase
Al
L + Nb3Al Ð NbNi
1635
p3
L
L + NbNi Ð Nb10Ni9Al3
1615
p4
L Ð NbNi + NbNiAl
1571
L Ð NiAl + NbNiAl
Nb
Ni
29.68
50.56
19.76
L
24.6
45.10
30.30
e1
L
37.42
39.09
23.49
1460
e3
L
37.06
18.87
44.07
L Ð NbAl3 + NbNiAl
1419
e4
L
57.5
31.25
11.25
L Ð NbNi3 + NbNiAl
1276
e7
L
7.28
29.96
62.76
L Ð NbNi3 + Ni3Al
1275
e8
L
11.32
15.44
73.24
L Ð NbNiAl + Ni3Al
1204
e9
-
-
-
-
NiAl + NbNiAl Ð NbNi2Al
1178
p7
-
-
-
-
Nb10Ni9Al3 Ð NbNiAl +NbNi
910
e11
-
-
-
-
NbNi Ð NbNi2Al + (Nb)
815
e12
-
-
-
-
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Table 5 Thermodynamic Properties of Single Phases Temperature Range [˚C]
Phase
Property, per mole of atoms [J, mol, K]
Comments
τ1, Al25Ni50Nb25
25
–38600 ± 1100
Enthalpy of formation [2006Hu]
τ2, Al27Ni40Nb33:
25
–39600 ± 1600
Enthalpy of formation [2006Hu]
τ2, Al33.3Ni33.3Nb33.3
25
–40900 ± 1500
Enthalpy of formation [2006Hu]
τ2, Al40Ni20Nb33: (N.B. not 100%)
25
–46200 ± 1300
Enthalpy of formation [2006Hu]
NiAl3 of composition: Al75Ni17Nb8
25
–40300 ± 1100
Enthalpy of formation [2006Hu]
Ni3Al of composition: Al20Ni76Nb4
25
–28400 ± 800
Enthalpy of formation [2006Hu]
. Table 6 Investigations of the Al-Nb-Ni Materials Properties Reference
Method / Experimental Technique
Type of Property
[1967Arb]
Hardness, mechanical testing
Vickers Hardness, Young’s modulus, thermal expansion
[1978Sve, 2006Gre]
TEM
Dislocation structures
[1980Bhe, 1991Gra]
Thermogravimetric analysis
Oxidation behavior, oxidation rates
[1984Tor]
Metallography, directional solidification, mechanical testing
Phases, high temperature strength, fracture toughness
[1991Laa]
HIP poweder compacts, mechanical testing
Young’s modulus, Poisson’s ratio, and fracture toughness at RT
[1991Och]
Compression testing
Stress-strain behavior
[1992Gra]
Thermogravimetric analysis
Oxidation resistance of intermetallic phases
[1992Rev]
Directional solidification, microhardness
Microhardness and fracture strength
[1993He]
Thermogravimetric analysis
Corrosion behavior
[1993Rei]
Compression testing
High temperature strength, fracture toughness
[1996Mac]
Mechanical testing
Deformation behaviour of τ2, NbNiAl
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
13
14
11
Al–Nb–Ni
. Table 6 (continued) Reference
Method / Experimental Technique
[1998Far]
Solid state sintering of elemental powders; Hardness testing, compression testing
NiAl-Nb composites; Hardness testing, compression testing
[1999Roc]
Calorimetry
Low temperature specific heat
[2002Kim]
Metallography, DTA
Phase transformations
[2002Rio]
Hardness testing
Hardness, fracture toughness
[2003Cer1, 2003Cer2]
Diffusion couples
Interdiffusion coefficients
[2006Bel]
Creep testing
Creep strength
[2006Hag]
Three-point bending
Fracture toughness
[2006Rin]
Velocity of elastic waves
Elastic modulus
[2006Yu]
Compression testing
Fabrication and characterization of Ni-Nb particle-reinforced Al-based composite
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Type of Property
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 1 Al-Nb-Ni. Adopted binary Nb-Ni system
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
15
16
11
Al–Nb–Ni
. Fig. 2 Al-Nb-Ni. Experimental quasibinary system between NiAl and τ2 ( NbNiAl)
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
11
. Fig. 3a Al-Nb-Ni. Reaction scheme, part 1
Al–Nb–Ni
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
17
11
Al–Nb–Ni
. Fig. 3b Al-Nb-Ni. Reaction scheme, part 2
18
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
11
. Fig. 3c Al-Nb-Ni. Reaction scheme, part 3
Al–Nb–Ni
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
19
20
11
Al–Nb–Ni
. Fig. 4 Al-Nb-Ni. Liquidus surface projection
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 5 Al-Nb-Ni. Experimental liquidus lines in the Ni-rich corner between 1325 and 1450˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
21
22
11
Al–Nb–Ni
. Fig. 6 Al-Nb-Ni. Experimental solidus lines in the Ni-rich corner between 1325 and 1450˚C
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 7 Al-Nb-Ni. Dependence of the solvus line of (Ni) on Al concentration
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
23
24
11
Al–Nb–Ni
. Fig. 8 Al-Nb-Ni. Isothermal section at 1300˚C
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 9 Al-Nb-Ni. Isothermal section at 1200˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
25
26
11
Al–Nb–Ni
. Fig. 10 Al-Nb-Ni. Isothermal section at 1140˚C
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 11 Al-Nb-Ni. Isothermal section at 1080˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
27
28
11
Al–Nb–Ni
. Fig. 12 Al-Nb-Ni. Isothermal section at 1027˚C
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 13 Al-Nb-Ni. Isothermal section at 900˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
29
30
11
Al–Nb–Ni
. Fig. 14a Al-Nb-Ni. Isothermal section at 800˚C, Ni rich corner
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 14b Al-Nb-Ni. Isothermal section at 800˚C, Al rich corner
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
31
32
11
Al–Nb–Ni
. Fig. 15 Al-Nb-Ni. Isothermal section at 750˚C
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
. Fig. 16 Al-Nb-Ni. Isothermal section at 600˚C
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
33
34
11
Al–Nb–Ni
. Fig. 17 Al-Nb-Ni. Experimental temperature - composition section Ni3Al - NbNi3
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni
11
References [1962Arb]
[1962Min1]
[1962Min2]
[1963Arb] [1964Sch] [1965Gol]
[1965Kor]
[1965Mar]
[1965Ram]
[1966Ben] [1966Mar]
[1967Arb]
[1967Sho] [1968Hun]
[1969Gus]
[1969Nov]
[1969Tho]
[1970Cis] [1970Duv]
Arbuzov, M.P., Chuprina, V.G., “X-Ray Determination of the Crystal Structures of Alloys in the Ni3AlNi3Nb System” (in Russian), Akad. Nauk SSSR, Inst. Metall. Im A.A. Baikova, (8), 85–87 (1962) (Crys. Structure, Experimental, 13) Mints, R.S., Belyaeva, G.F., Malkov, Yu.S., “The Reaction Between the Metallic Compounds Ni3Al and Ni3Nb” (in Russian), Dokl. Akad. Nauk SSSR, 143(4), 871–874 (1962) (Phase Relations, Phase Diagram, *, 26) Mints, R.S., Belyaeva, G.F., Malkov, Y.S., “Equlibrium Diagram of the Ni3Al-Ni3Nb System”, Russ. J. Inorg. Chem. (Engl. Transl.), 7, 1236–1239 (1962), translated from Zh. Neorg. Khim., 7(10), 2382–2385 (1962) (Experimental, Morphology, Phase Relations, *, 32) Arbuzov, M.P., Chuprina, V.G., “Ageing Alloys of the System Ni3Al-Ni3Nb” (in Russian), Izv. V. U. Z., Fiz., 5, 82–85 (1963) (Crys. Structure, Phase Diagram, Experimental, *, 2) Schubert, K., Meissner, H.G., Raman, A., Rossteutscher, W., “Structural Data of Some Metallic Phases”, Naturwissenschaften, 51, 287 (1964) (Crystal Structure, 0) Golubtsova, R.B., “Selective Isolation of Metallic Compounds from an Alloy of the Ni3Al-Ni3Nb System” (in Russian), Dokl. Akad. Nauk SSSR, 160, 1311–1314 (1965) (Experimental, Phys. Prop., Kinetics, 13) Kornilov, I.I., Mints R.S., Guseva, L.N., Malkov, Y.S., “Interaction Between the Compound NiAl and Niobium”, Russ. Metall. (Engl. Transl.), (6), 93–96 (1965), translated from Izv. Akad. Nauk SSSR, Met., (6), 132–136 (1965) (Experimental, Morphology, Phase Diagram, Phase Relations, #, 5) Markiv, V.Ya., Voroshilov, Yu.V., Kripyakevich, P.I., Cherkashin, E.E., “New Compounds of the MnCu2Al and MgZn2 Types Containing Aluminum and Gallium”, Sov. Phys. Crystallogr., 9, 619–620 (1965) translated from Kristallografiya, 9, 737–738 (1964) (Crys. Structure, Experimental, 4) Raman, A., Schubert, K., “On the Crystal Structure of Some Alloy Phases Related to TiAl3. III. Investigations in Several T-Ni-Al and T-Cu-Al Systems” (in German), Z. Metallkd., 56, 99–104 (1965) (Crys. Structure, Experimental, Phase Diagram, 14) Benjamin, J.S., Giessen, B.C., Graut, N.J., “Intermediate Phases in the Ternary System Nb(Cb)-Ni-Al at 1140˚C”, Trans. Metall. Soc. AIME, 236, 224–226 (1966) (Experimental, Phase Relations, #, 8) Markiv, V.Ya., Matushevskaya, N.F., Kuz’ma, Yu.B., “X-Ray Diffraction of the Nb-Ni-Al System”, Russ. Metall. (Engl. Transl.), (6), 72–74 (1966), translated from Izv. Akad. Nauk SSSR, Met., (6), 127–129 (1966) (Experimental, Phase Relations, *, 2) Arbuzov, M.P., Chuprina, V.G., “Determination of Some Physical Properties of the Ni3Al-Ni3Nb Alloys”, Russ. Metall. (Engl. Transl.), (3), 78–80 (1967), translated from Izv. Akad. Nauk SSSR, Met., (3), 174–179 (1967) (Experimental, Phase Relations, Phys. Prop., 7) Shoemaker, C.B., Shoemaker, D.P., “The Crystal Structure of the M Phase, NbNiAl”, Acta Crystallogr., 23, 231–238 (1967) (Crys. Structure, Experimental, 18) Hunt, C.R. Jr., Raman, A., “Alloy Chemistry of σ (βαffl U)-Related Phases. I. Extens Ion of μ- and Occurrence of μ’-Phases in the Ternary Systems Niobium(Tantalum)-X-Aluminum X = Iron, Cobalt, Nickel, Copper, Chromium, Molybdenum)”, Z. Metallkd., 59(9), 701–707 (1968) (Crys. Structure, Phase Diagram, *, 14) Guseva, L.N., Mints, R.S., Malhov, Y.S., “Phase Equilibria in the Ni-Ni3Al-Ni3Nb System at 800–1200˚C”, Russ. Metall. (Engl. Transl.), (5), 120–122 (1969), translated from Izv. Akad. Nauk SSSR, Met., (5), 186–188 (1969) (Experimental, Phase Relations, *, 12) Novic, F.S., Mints, R.S., Malkov, Yu.S., “Plotting the Liquidus Surface of a Ni-Ni3Al-Ni3Nb Ternary System” (in Russian) in “Teor. Eksp. Metody Issled. Diagramm Sostoyaniya Metal. Sistem”, Ageev, N.V. (Ed.), Nauka, Moscow, 145–150 (1969) (Phase Diagram, Experimental, *, 10) Thompson, E.R., Lemkey, F.D., “Structure and Properties of Ni3Al Eutectic Alloys Produced by Unidirectional Solidification”, Trans. Quart., A.S.M., 62, 140–154 (1969) (Phase Diagram, Experimental, *, 35) Cisse, J., Davies, R.G., “Nickel-Rich Portion of the Nickel-Aluminum-Niobium Phase Diagram”, Met. Trans., 1, 2003–2006 (1970) (Experimental, Mechan. Prop., Morphology, Phase Diagram, 9) Duvall, D.S., Donachie, M.J., “Phase Equilibria in Nickel-Rich Ni-Al-Nb Alloys”, J. Inst. Met., 96, 182–187 (1970) (Experimental, Morphology, Phase Diagram, *, 16)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
35
36
11 [1971Min]
[1972Duv] [1973Kra]
[1973Lem]
[1973Wil] [1975Bok]
[1975Kau] [1975Kra]
[1978Gul] [1978Sve]
[1979Oma]
[1980Bhe]
[1980Jor]
[1980Nas] [1983Och] [1984Arg] [1984Bre] [1984Lia] [1984Och1]
[1984Och2] [1984Tor]
Al–Nb–Ni Mints, R.S., Malkov, Y.S., Davydor, N.I., Kofanova, G.N., “Polythermal Sections of the Ni-Ni3Al-Ni3Nb System at Nb 5 and 10 wt.-%” (in Russian), Diagrammy Sost. Metall. Sistem, 158–160 (1971) (Phase Diagram, Phase Relations, Experimental, Mechan. Prop., 8) Duvall, D.S., Donachie, M.J. Jr., “Precipitation Characteristics of Nickel-Rich Ni-Al-Nb Alloys”, J. Inst. Met., 100, 6–12 (1972) (Experimental, Morphology, Phase Relations, 22) Kraft, E.H., Thompson, E.R., “Directional Solidification of Ni-Nb, Ni-Al-Nb, Ni-Cr-Nb and Ni-Cr-AlNb Alloys”, Proc. Conf. “In Situ Composites”, National Academy of Science, Washington, 297–303 (1973) (Phase Relations, Experimental, *, 18) Lemkey, F.D., Thompson, E.R., “Eutectic Superalloys Strengthened by Aligned S-Ni3Nb Lamellas, γ’(Ni3Al) Precipitates and Reduced Interlamellar Spacing”, Proc. Conf. “In Situ Composites”, National Academy of Science, Washington, 161 (1973) (Phase Relations, Experimental) Willey, L.A., “The Al-Nb System” in “Metals Handbook”, 8th Ed., Vol. 8, ASM, Metals Park Ohio, 342 (1973) (Phase Relations, Review, #, 3) Bokshteyn, S.Z., Vasilenok, L.B., Kishkin, S.T., Nazarova, M.P., Svetlov, I.L., Sorokina, L.P., Khusnetdinov, F.M., “Formation of the Eutectic γ/γ’ - δ Microstructure During Directional Crystallization and After Heat Treatment”, Phys. Met. Metallogr., 79–85 (1975) (Experimental, Morphology, Phase Diagram, 17) Kaufman, L., Nesor, H., “Calculation of Superalloy Phase Diagrams. Part III”, Metall. Trans. A, 6(11), 2115–2122 (1975) (Calculation, Crys. Structure, Phase Diagram, Thermodyn., 35) Kraft, E.H., Thompson, E.R., “Directional Solidification of Ni-Nb, Ni-Al-Nb, Ni-Cr-Nb and Ni-Cr-AlNb Alloys”, 2nd Conf. on in Situ Composites, Boston, 297–307 (1975) (Experimental, Thermodyn., Phase Relations, 18) Gulyaev, B.B., Grigorash, E.F., Efimova, M.N., “Solidification Range of Ni Alloys”, Met. Sci. Heat Treat., 20, 914–917 (1978) (Experimental, Phase Relations, 8) Svetlov, I.L., Vasilenok, L.B., Khusnetdinov, F.M., Sidorov, V.V., Nazarova, M.P., “Plastic Deformation of Directionally Crystallized Eutectic Ni/Ni3Al-Ni3Nb”, Phys. Met. Metallogr., 45(1), 124–129 (1978) (Experimental, Mechan. Prop., 12) Omarov, A.K., Smagulov, S.U., Askarov, M.S., “Study of Phase Equilibriums in Alloys of Al-Ni-Zn and Al-Nb-Ni Ternary Systems” (in Russian), Metall. Obogashch., 133–137 (1979) (Abstract, Experimental, Phase Diagram, Phase Relations, 5) Bhedwar, H.C., Heckel, R.W., Laughlin, D.E., “The Oxidation Behavior of Aluminide-Coated γ/δ Directional Eutectics”, Metall. Trans. A, 11, 1303–1314 (1980) (Experimental, Mechan. Prop., Morphology, Phase Diagram, Phase Relations, Phys. Prop., 25) Jorda, J.L., Fluekiger, R., Mueller, J., “A New Metallurgical Investigation of the NiobiumAluminium System”, J. Less-Common Met., 75, 227–239 (1980) (Crys. Structure, Phase Diagram, Experimental, #, 20) Nash, P., Kavishe, F.P.L., West, D.R.F., “Nickel-Rich Region of Ni-Al-Nb System at 1473 K”, Met. Sci., 14(4), 147–149 (1980) (Experimental, Phase Relations, Crys. Structure, *, 21) Ochiai, S., Oya, Y., Suzuki, T., “Solubility Data in Ni3Al with Ternary Additions”, Bull. P.M.E. (T.I.T.), 52, 1–17 (1983) (Phase Diagram, Experimental, 45) Argent, B.B., “Phase Diagrams of Alloys Based on Niobium”, Metals Society/AIME Acc. No. 84(7), 72–486, 325–415 (1984) (Crys. Structure, Phase Diagram) Brezovsky, M., “Morphology of Eutectic Composite Material γ-γ´”, Kovove Mater., 1 (22), 104–112 (1984) (in Slovakija) (Experimental, 17) Liang, W.W., Standley, R., Nash, P., Skowron, M., “The Relative Stabilities of the Ni6AlX (X = V, Nb, Ta) Phases”, J. Mater. Sci. Lett., 3(3), 259–261 (1984) (Experimental, 5) Ochiai, S., Mishima, Y., Suzuki, T., “Lattice Parameter Data of Ni (γ), Ni3Al (γ’) and Ni3Ga (γ’) Solid Solutions”, Bull. Res. Lab. Precis. Machin. Electron., Tokyo Inst. Technol., 53, 15–28 (1984) (Crys. Structure, Experimental, *, 66) Ochiai, S., Oya, Y., Suzuki, T., “Alloying Behaviour of Ni3Al, Ni3Ga, Ni3Si and Ni3Ge”, Acta Metall., 32(2), 289–298 (1984) (Experimental, Phase Diagram, 90) Toropov, V.M., Bondarenko, Yu.A., “Properties of High-Temperature Alloys of the System Ni-Al-Nb with a Unidirectional Eutectic Structure”, Met. Sci. Heat Treat., 26(9-10), 660–664 (1984), translated from Metalloved. Term. Obrab. Met., (9), 11–15, 1984 (Experimental, Mechan. Prop., Phase Diagram, 8)
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
MSIT1
Landolt‐Bo¨rnstein New Series IV/11E1
Al–Nb–Ni [1985Mis]
[1985Mor] [1985Tro] [1986Bla] [1987Akh] [1988Mor]
[1989Hon] [1989Sub]
[1991Eno]
[1991Gra]
[1991Ino] [1991Laa]
[1991Mis] [1991Och]
[1991Sas]
[1991Ska]
[1992Gra]
[1992Lee] [1992Rev]
[1993He]
[1993Rei]
11
Mishima, Y., Ochiai, S., Suzuki, T., “Lattice Parameters of Ni(γ), Ni3Al(γ’) and Ni3Ga(γ’) Solid Solutions with Additions of Transition and B-Subgroup Elements”, Acta Metall., 33(6), 1161–1169 (1985) (Experimental, 64) Morinaga, M., Yukawa, N., Ezaki, H., Adachi, H., “Solid Solubilities in Nickel-Based F.C.C. Alloys”, Philos. Mag. A, 51(2), 247–252 (1985) (Phase Diagram, Phase Relations, Experimental, 26) Trojko, R., Blazina, Z., “Metal-Metalloid Exchange in Some Friauf-Laves Phases Containing Two Transition Metals”, J. Less-Common Met., 106, 293–300 (1985) (Crys. Structure, Experimental, 13) Blazina, Z., Trojko, R., “Structural Investigations of the Nb(1–x)SixT2 and Nb(1–x)AlxT2 (T = Cr, Mn, Fe, Co, Ni) Systems”, J. Less-Common Met., 119, 297–305 (1986) (Crys. Structure, Experimental, 6) Akhtar, D., Misra, R.D.K., “Formation and Stability of Ni60Nb40-xAlx”, J. Mater. Sci. Lett., 6(1), 29–30 (1987) (Experimental, 19) Morinaga, M., Sone, K., Kamimura, T., Ohtaka, K., Yukawa, N., “X-Ray Determination of Static Displacements of Atoms in Alloyed Ni3Al”, J. Appl. Crystallogr., 21, 41–46 (1988) (Crys. Structure, Experimental, 18) Hong, Y.M., Mishima, Y., Suzuki, T., “Accurate Determination of γSolvus in Ni-Al-X Ternary Systems”, Mater. Res. Soc. Symp. Proc., 133, 429–440 (1989) (Experimental, Phase Diagram, Phase Relations, 35) Subramanian, P.R., Simmons, J.P., Mendiratta, M.G., Dimiduk, D.M., “Effect of Solutes on Phase Stability in Al3Nb”, Mater. Res. Soc. Symp. Proc., 133(3), 51–56 (1989) (Experimental, Mechan. Prop., Phase Diagram, 12) Enomoto, M., Harada, H., Yamazaki, M., “Calculation of γ’/γ Equilibrium Phase Compositions in Nickel-Base Superalloys by Cluster Variation Method”, Calphad, 15(2), 143–158 (1991) (Assessment, Calculation, Phase Diagram, 34) Grabke, H.J., Steinhorst, M., Brumm, M., Wiemer, D., “Oxidation and Intergranular Disintegration of the Aluminides NiAl and NbAl3 and Phases in the System Nb-Ni-Al”, Oxid. Met., 35(3-4), 199–222 (1991) (Electronic Structure, Experimental, Kinetics, Thermodyn., 30) Inoue, H.R.P., Kitamura, M., Wayman, C.M., Chen, H., “Phase Stability of Al3Nb as a Function of Nickel Additions”, Philos. Mag. Lett., 63(6), 345–353 (1991) (Crys. Structure, Experimental, 19) Laag, R., Kaysser, W.A., Petzow, G., “A Comparative Study on the Influence of Nb and Ti Additions to Different Processed Atomized NiAl Powders”, Mater. Res. Soc. Symp. Proc.: High-Temp. Ordered Intermetallic Alloys IV, 213, 821–826 (1991) (Experimental, Mechan. Prop., 9) Mishima, Y., Hong, Y.M., Suzuki, T., “Determination of the γ Solvus Surface in Ni-Al-X Ternary Systems”, Mater. Sci. Eng. A, 146, 123–130 (1991) (Assessment, Experimental, Phase Diagram, 5) Ochiai, S., Shirokura, T., Doi, Y., Kojima, Y., “Microstrucutres and Mechanical Properties of Ni-Nb Aluminides Produced by MA Process”, ISIJ Int., 31(10), 1106–1112 (1991) (Experimental, Mechan. Prop., 27) Sasaki, K., Morinaga, M., Yukawa, N., “Alloying Effect on thr Solidified Structure of NiAl”, Proc. Conf. Intermetal. Comp. - Struct. Mechan. Prop., 877–881 (1991) (Abstract, Experimental, Mechan. Prop., Phase Diagram, 10) Skakov, Yu.A., Djakonova, N.P., Edneral, N.V., Koknaeva, M.R., Semina, V.K., “Some Peculiarities of the Atomic Structure of Metallic Phase Formed During Liguid Quenching and Solid State Reactions”, Mater. Sci. Eng. A, 133, 560–564 (1991) (Experimental, Phase Relations, 5) Grabke, H.J., Brumm, M., Steinhorst, M., “Development of Oxidation Resistant High Temperature Intermetallics”, Mater. Sci. Technol., 8, 339–344 (1992) (Experimental, Interface Phenomena, Phase Diagram, Thermodyn., 21) Lee, K.J., Nash, P., “The Al-Nb-Ni System”, to be published in J. Phase Equilib., (Crys. Structure, Phase Diagram, Review, #, 27) a copy is available at MSI Reviere, R.D., Noebe, R.D., Oliver, B.F., “Processing, Microstructure and Low-Temperature Properties of Directionally Solidified NiAl/NiAlNb Alloys”, Mater. Lett., 14(2-3), 149–155 (1992) (Morphology, Phase Relations, Mechan. Prop., 19) He, Y.R., Douglass, D.L., “The Corrosion Behavior of Ni-Al Alloys and Ni-Nb-Al Alloys in a H2/H2O/ H2S Gas Mixture”, Oxid. Met., 40(3-4), 337–371 (1993) (Experimental, Kinetics, Morphology, Phase Relations, 28) Reip, C.-P., Sauthoff, G., “Deformation Behaviour of the Intermetallic Phase Al3Nb with DO22 Structure and of Al3Nb-base Alloys: Part 1. Physical Properties and Short-Term Behaviour”, Intermetallics, 1, 159–169 (1993) (Experimental, Phase Diagram, Phys. Prop., 30)
Landolt‐Bo¨rnstein New Series IV/11E1
MSIT1
DOI: 10.1007/978-3-540-88053-0_11 ß Springer 2009
37
38
11 [1993Sau]
[1994Jia]
[1995Net] [1996Mac] [1996Rav]
[1997Uey]
[1998Far]
[1999Roc]
[2000Boz] [2000DeL]
[2000Rio] [2001Kai]
[2001Miu]
[2001Sav]
[2001Son] [2001Ter]
[2002Boz] [2002Kim]
[2002Kri]
[2002Rio]
Al–Nb–Ni Saunders, N., “Aluminium - Niobium - Nickel”, MSIT Ternary Evaluation Program, in MSIT Workplace, Effenberg, G. (Ed.), MSI, Materials Science International Services GmbH, Stuttgart; Document ID: 10.10206.1.20, (1993) (Crys. Structure, Phase Diagram, Assessment, XX) Jia, C.C., Ishida, K., Nishizawa, T., “Partition of Alloying Elements Between γ (A1), γ’ (L12) and β (B2) Phases in Ni-Al Base Systems”, Metall. Mater. Trans. A, 25, 473–485 (1994) (Crys. Structure, Experimental, Phase Diagram, 25) Neto, R.M.L., Ferreira, P.I., “Reaction Sintering of Nb-Ni-Al Intermetallic Alloys”, Mater. Sci. Eng. A, 193, 549–555 (1995) (Experimental, Kinetics, Mechan. Prop., Phase Relations, Thermodyn., 18) Machon, L., Sauthoff, G., “Deformation Behaviour of Al-Containing C14 Laves Phase Alloys”, Intermetallics, 4, 469–481 (1996) (Experimental, Phase Relations, 41) Ravindran, P., Subramoniam, G., Asokamani, R., “Ground-State Properties and Relative Stability Between the L12 and Doa Phases of Ni3Al by Nb Substitution”, Phys. Rev. B, 53(3), 1129–1137 (1996) (Calculation, Crys. Structure, Thermodyn., 44) Ueyama, T., Ghanem, M.M., Miura, N., Takeyama, M., Matsuo, T., “Phase Stability of Ni3Nb-δ Phase in Ni-Nb-M Systems at Elevated Temperatures”, THERMEC´97, Intern. Conf. Thermomechan. Proc. Steels Other Mater., TMS, Warrendale, USA, 2, 1753–1760 (1997) (Crys. Structure, Experimental, Morphology, Phase Diagram, Phase Relations, 16) Farber, L., Gotman, I., Gutmanas, E.Y., Lawley, A., “Solid State Synthesis of NiAl-Nb Composites from Fine Elemental Powders”, Mater. Sci. Eng. A, 244(1), 97–102 (1998) (Experimental, Morphology, Phase Relations, 29) da Rocha, F.S., Fraga, G.L.F., Brandao, D.E., da Silva, C.M., Gomes, A.A., “Specific Heat and Electronic Structure of Heusler Compounds Ni2Tal (T = Ti, Zr, Hf, V, Nb, Ta)”, Physica B (Amsterdam), 269, 154–162 (1999) (Crys. Structure, Experimental, 20) Bozzolo, G., Noebe, R.D., Honecy, F., “Modeling of Ternary Element Site Substitution in NiAl”, Intermetallics, 8, 7–18 (2000) (Crys. Structure, Review, 34) De Lima, B.B., Ramos, A.S., Nunes, C.A., Conte, R.A., “Ni-65 wt.% Nb Alloy by Aluminothermic Reduction Process”, Int. J. Refract. Met. Hard Mater., 18, 267–271 (2000) (Experimental, Phase Diagram, 6) Rios, C.T., Milenkovic, S., Caram, R., “Directional Growth of Al-Nb-X Eutectic Alloys”, J. Cryst. Growth, 211, 466–470 (2000) (Experimental, Phase Relations, 8) Kainuma, R., Ichinose, M., Ohnuma, I., Ishida, K., “Formation of γ´/β Interface Morphologies in Ni-Al-X Ternary Diffusion Couples”, Mater. Sci. Eng. A, 312, 168–175 (2001) (Experimental, Phase Relations, Thermodyn., 21) Miura, S., Hong, Y.-M., Suzuki, T., Mishima, Y., “Li