Cover
title author publisher isbn10 | asin print isbn13 ebook isbn13 language subject publication date lcc ddc subject
: : : : : : : : : : :
Nanostructured Silicon-based Powders and Composites Legrand, A. P.; Senemaud, C. CRC Press 9780203297551 9780203222294 English Nanostructures, Silicon--Industrial applications. 2003 QC176.8.N35N36 2003eb 620.5 Nanostructures, Silicon--Industrial applications.
cover
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/cover.html [20/01/2010 10:02:55 AM]
page_i
< previous page
page_i
next page >
Page i Nanostructured Silicon-based Powders and Composites
< previous page
page_i
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_i.html [20/01/2010 10:02:56 AM]
page_ii
< previous page
page_ii
next page >
page_ii
next page >
Page ii This page intentionally left blank.
< previous page
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_ii.html [20/01/2010 10:02:56 AM]
page_iii
< previous page
page_iii
next page >
Page iii Nanostructured Silicon-based Powders and Composites Edited by André P. Legrand and Christiane Sénémaud
LONDON AND NEW YORK
< previous page
page_iii
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_iii.html [20/01/2010 10:02:56 AM]
page_iv
< previous page
page_iv
next page >
Page iv First published 2003 by Taylor & Francis 11 New Fetter Lane, London EC4P 4EE Simultaneously published in the USA and Canada by Taylor & Francis Inc, 29 West 35th Street, New York, NY 10001 Taylor & Francis is an imprint of the Taylor & Francis Group This edition published in the Taylor & Francis e-Library, 2003. © 2003 Taylor & Francis All rights reserved. No part of this book may be reprinted or reproduced or utilised in any form or by any electronic, mechanical, or other means, now known or hereafter invented, including photocopying and recording, or in any information storage or retrieval system, without permission in writing from the publishers. Every effort has been made to ensure that the advice and information in this book is true and accurate at the time of going to press. However, neither the publisher nor the authors can accept any legal responsibility or liability for any errors or omissions that may be made. In the case of drug administration, any medical procedure or the use of technical equipment mentioned within this book, you are strongly advised to consult the manufacturer’s guidelines. British Library Cataloguing in Publication Data A catalogue record for this book is available from the British Library Library of Congress Cataloging in Publication Data A catalog record for this book has been requested ISBN 0-203-22229-6 Master e-book ISBN ISBN 0-203-29755-5 (OEB Format) ISBN 0-415-30113-0 (Print Edition) Cover: A laser irradiation cell observed through a KCl window
< previous page
page_iv
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_iv.html [20/01/2010 10:02:57 AM]
page_v
< previous page
page_v
next page >
Page v
Christiane Sénémaud was a CNRS Directeur de Recherches until she passed away in 1998. Her area of expertise was the determination of the electronic structure of complex materials by X-ray photoelectrons and soft X-ray spectroscopies. She had published more than one hundred papers and communications in international meetings, and owing to her open mind and vast knowledge, she skilfully established fruitful cooperation between foreign and French laboratories. Moreover, she directed the theses of many young students and contributed to graduate education at the university, more precisely the ‘Complex Materials’ doctoral school. Finally, she was the leader of the CNRS research group that was the origin of this book. Her merit was recognised with the attribution of the Charles-Louis de Saulces de Freycinet Award by the French Academy of Sciences. Christiane Sénémaud was above all smart, discrete, fair, active, efficient and kind. For these reasons, the authors would like to dedicate this book to her memory.
< previous page
page_v
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_v.html [20/01/2010 10:02:57 AM]
page_vi
< previous page
page_vi
next page >
page_vi
next page >
Page vi This page intentionally left blank.
< previous page
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_vi.html [20/01/2010 10:02:58 AM]
page_vii
< previous page
page_vii
next page >
Page vii Contents List of contributors Foreword Preface Acknowledgements 1 Objectives and state-of-the-art of nanocomposites MICHEL CAUCHETIER AND ANDRÉ PIERRE LEGRAND 1.1 Introduction 1.2 Nanostructured ceramic elaboration 1.3 Nanostructured Si3N4/SiC materials 1.4 Analytical methods 1.5 Conclusion References 2 Laser synthesis of nanosized powders MICHEL CAUCHETIER, EMMANUEL MUSSET, MICHEL LUCE, NATHALIE HERLIN, XAVIER ARMAND AND MARTINE MAYNE 2.1Generalities on the synthesis of nanosized powders by laser pyrolysis 2.2 Synthesis of Si, SiC, Si3N4and SiC—Si3N4mixtures with SiH4and SiH3CH3as silicon precursors 2.3 Synthesis of silicon carbonitride (Si/C/N) powders using hexamethyldisilazane as Si precursor 2.4 Silicon carbonitride (Si/C/N) powders containing in situ the elements of the sintering aids (Al, Y): pre-mixed powders 2.5 Conclusion References 3 Thermal behaviour of as-formed silicon-based nanopowders
< previous page
page_vii
xi xiii xv xvi 1
1 2 3 4 5 5 6 6 8 15 19 22 23 25
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_vii.html [20/01/2010 10:02:58 AM]
page_viii
< previous page
page_viii
next page >
Page viii 3.1 Thermal behaviour in a high-temperature graphite furnace EMMANUEL MUSSET, MARTINE MAYNE, MICHEL CAUCHETIER, XAVIER ARMAND, MICHEL LUCE AND NATHALIE HERLIN-BOIME 3.1.1 Introduction 3.1.2 Weight evolution of SiC, Si/C/N and Si/C/N/Al/Y/O nanopowders 3.1.3 Chemical evolution during annealing in a nitrogen atmosphere 3.1.4 Structural changes 3.1.5 Information about changes in the grain sizes 3.1.6 Conclusion References 3.2 Thermal reactivity of silicon-based nanopowders DJAMILA BAHLOUL-HOURLIER, BENOÎT DOUCEY, JEAN-LOUIS BESSON AND PAUL GOURSAT 3.2.1 Introduction 3.2.2 Results and discussions 3.2.3 Conclusion References 4 Structure of some nanopowders and micro/nano composites by transmission electron microscopy MARC MONTHIOUX, CATHERINE BÉRAUD AND NAHIDA EL HORR 4.1 As-prepared and heat-treated nanopowders 4.2 As-prepared sintered composites 4.3 TEM sample preparation prior to investigations and operating conditions References 5 From short- to long-range order 5.1 Chemical order studied by solid-state nuclear magnetic resonance ANDRÉ PIERRE LEGRAND, JEAN-BAPTISTE D’ESPINOSE DE LA CAILLERIE AND YOUSSEF EL KORTOBI 5.1.1 Nuclear magnetic methods 5.1.2 SiC powders analysis 5.1.3 Si/C/N powders analysis 5.1.4 Pre-alloyed Si/C/N/Al/Y nanopowders 5.1.5 Conclusion References
< previous page
page_viii
26
26 26 29 33 39 40 40 41 41 42 53 53 54 54 95 105 109 110 111 111 115 119 129 137 138
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_viii.html [20/01/2010 10:02:59 AM]
page_ix
< previous page
page_ix
next page >
Page ix 5.2 Paramagnetic defect states in silicon-based nanopowders ABDELHADI KASSIBA AND STÉPHANE CHARPENTIER 5.2.1Introduction 5.2.2 Theoretical background 5.2.3 Experimental details 5.2.4 Si/C powders 5.2.5 Assignment of the paramagnetic species in Si/C nanopowders 5.2.6 Silicon carbonitride (Si/C/N) powders References 5.3 Electronic structure studied by X-ray photoemission (XPS) and soft-X-ray (SXS) spectroscopies ADRIANA GHEORGHIU DE LA ROCQUE, GEORGES DUFOUR, FRANÇOIS TÉNÉGAL AND CHRISTIANE SÉNÉMAUD 5.3.1Principles 5.3.2 Experiments 5.3.3 Study by XPS–SXS of Si, Si/C, Si/N and Si/C/N laser synthetised nanopowders produced from gaseous precursors 5.3.4 Effect of heat treatment on the electronic structure of nanometric Si/C/N ex-HMDS and prealloyed Si/C/N/Al/Y powders studied by XPS spectroscopy References 5.4 Local order in Si/C/N nanopowders studied by X-ray absorption spectroscopy: study at the Si—K edge FRANÇOIS TÉNÉGAL, ANNE-MARIE FLANK, ADRIANA GHEORGHIU-DE LA ROCQUE AND CHRISTIANE SÉNÉMAUD 5.4.1 X-ray absorption principles and data analysis 5.4.2 Study by EXAFS at the Si—K edge of Si, SiN, SiC and Si/C/N laser-synthetised nanopowders produced from gaseous precursors 5.4.3 Short-range order determination in amorphous SiCN-HMDS nanopowders: evolution as a function of the C/N ratio and annealing treatment 5.4.4 Local structure of pre-alloyed Si/C/N/Al/Y nanopowders studied by XAS at the Al—K edge using fluorescence yield detection References 5.5 Neutron and X-ray diffraction applied to the study of the medium-range order in SiCN nanopowders FRANÇOIS TÉNÉGAL, BRIGITTE BOUCHET-FABRE, JEAN DIXMIER AND ROBERT BELLISSENT 5.5.1Diffraction applied to the study of disordered compounds
< previous page
page_ix
139
139 140 141 141 144 146 152 153
153 154 155 165 180 182
182 187 192 205 209 211 211
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_ix.html [20/01/2010 10:02:59 AM]
page_x
< previous page
page_x
next page >
Page x 5.5.2 Early stages of the crystallisation of Si/C/N-HMDS nanopowders studied by X-ray and neutron diffraction: Nano-ordered Si/C/N structures References 6 Conductivity and dielectric properties of Si/C nanopowders ABDELHADI KASSIBA 6.1Introduction 6.2 Material specifications 6.3 Experimental results and interpretation 6.4 Conclusion References 7 Processing and tailoring of Si/C/N-based nanocomposites PAUL GOURSAT, DJAMILA BAHLOUL-HOURLIER, BENOÎT DOUCEY AND MARTINE MAYNE 7.1Introduction 7.2 Sintering of silicon nitride with additives 7.3 Sintering of silicon carbide 7.4 Si3N4/SiC nanocomposites 7.5 Conclusion References 8 Mechanical properties JEAN-LOUIS BESSON 8.1 Room temperature properties 8.2 High-temperature properties 8.3 Conclusion References 9 Theoretical investigations of Si/C/N-based alloys FABIO FINOCCHI 9.1 Introduction 9.2 Simulations of Si/C and Si/N disordered alloys 9.3 Simulations of ternary Si/C/N systems References Index
< previous page
page_x
211 225 227 227 228 228 237 237 238 238 238 241 241 262 263 264 264 268 280 280 282 282 284 290 297 299
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_x.html [20/01/2010 10:03:00 AM]
page_xi
< previous page
page_xi
next page >
Page xi Contributors Xavier Armand Commissariat à l’Energie Atomique, Service des photons, atomes et molécules, Bat 522. 91191 Gif-sur-Yvette Cedex, France Robert Bellissent Laboratoire Léon Brillouin, CEA-Saclay, batiment 563, 91191 Gif-sur-Yvette Cedex, France Catherine Béraud Laboratoire de Physique de la Matière Condensée, INA,135 avenur de Raugueil, 31077 Toulouse Cedex, France Jean-Louis Besson SPCTS, UMR CNRS 6638, ENSCI, 47-73, avenue Albert Thomas, 87065 Limoges Cedex, France Brigitte Bouchet-Fabre Laboratoire d’Utilisation du Rayonnement Electromagnétique, Bat. 209, Centre Universitaire Paris-Sud, 91405 Orsay Cedex, France Michel Cauchetier Commissariat à l’Energie Atomique Service des photons, atomes et molécules, Bat 522. 91191 Gif-sur-Yvette Cedex, France Stéphane Charpentier Laboratoire de Physique de l’Etat Condensé, Université du Maine, Faculté des Sciences, Boulevard Olivier Messiaen, 72085 Le Mans Cedex, France Jean Dixmier Laboratoire de Physique du Solide, 1 place Aristide Briand, 92195 Meudon Cedex, France Benoît Doucey SPCTS, UMR CNRS 6638, Faculté desSciences, 123, avenue Albert Thomas, 87060 Limoges Cedex, France Georges Dufour UMR CNRS7614, Laboratoire de Chimie-Physique, Université Pierre et Marie Curie, 11 rue P. M. Curie, 75231 Paris Cedex 05, France Nahida El Horr CEMES, BP 4347, 29 rue Jeanne Marvig, 31055 Toulouse Cedex 4, France Youssef El Kortobi FRE CNRS2312, Laboratoire de Physique Quantique, Ecole Supérieure de Physique et de Chimie Industrielles de la Ville de Paris, 10, rue Vauquelin, 75231 Paris Cedex 05, France Fabio Finocchi UMR CNRS7588, Groupe de Physique des Solides, UPMC, 2, place Jussieu, 75251 Paris Cedex 05, France Anne-Marie Flank Laboratoire d’Utilisation du Rayonnement Electromagnétique, Bat. 209, Centre Universitaire Paris-Sud, 91405 Orsay Cedex, France
< previous page
page_xi
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_xi.html [20/01/2010 10:03:00 AM]
page_xii
< previous page
page_xii
next page >
Page xii Adriana Gheorghiu-de La Rocque UMR CNRS7614, Laboratoire de Chimie-Physique, Université Pierre et Marie Curie, 11, rue P.M. Curie, 75231 Paris Cedex 05, France Paul Goursat SPCTS, UMR CNRS 6638, Faculté des Sciences, 123, avenue Albert Thomas, 87060 Limoges Cedex, France Nathalie Herlin-Boime Commissariat à l’Energie Atomique, DSM/DRECAM/SPAM-Laboratoire Francis Perrin URA CNRS2453, Bat 522. 91191 Gif-sur-Yvette Cedex, France Djamila Bahloul-Hourlier SPCTS, UMR CNRS 6638, Faculté des Sciences, 123, avenue Albert Thomas, 87060 Limoges Cedex, France Abdelhadi Kassiba Laboratoire de Physique de l’Etat Condensé, Université du Maine, Faculté des Sciences, Boulevard Olivier Messiaen, 72085 Le Mans Cedex, France Jean-Baptiste d’Espinose de la Caillerie FRE CNRS2312, Laboratoire de Physique Quantique, Ecole Supérieure de Physique et de Chimie Industrielles de la Ville de Paris, 10, rue Vauquelin, 75231 Paris Cedex 05, France André Pierre Legrand FRE CNRS2312, Laboratoire de Physique Quantique, Ecole Supérieure de Physique et de Chimie Industrielles de la Ville de Paris, 10, rue Vauquelin, 75231 Paris Cedex 05, France Michel Luce Commissariat à l’Energie Atomique Service des photons, atomes et molécules, Bat 522. 91191 Gif-sur-Yvette Cedex, France Martine Mayne Commissariat à l’Energie Atomique, DSM/DRECAM/SPAM-Laboratoire Francis Perrin URA CNRS2453, Bat 522. 91191 Gif-sur-Yvette Cedex, France Marc Monthioux CEMES, BP 4347, 29 rue Jeanne Marvig, 31055 Toulouse Cedex 4, France Emmanuel Musset Commissariat à l’Energie Atomique, Service des photons, atomes et molécules, Bat 522. 91191 Gif-sur-Yvette Cedex, France Christiane Sénémaud UMR CNRS7614, Laboratoire de Chimie-Physique, Université Pierre et Marie Curie, 11, rue P.M. Curie, 75231 Paris Cedex 05, France François Ténégal Laboratoire d’Utilisation du Rayonnement Electromagnétique, Bat. 209, Centre Universitaire Paris-Sud, 91405 Orsay Cedex, France
< previous page
page_xii
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_xii.html [20/01/2010 10:03:00 AM]
page_xiii
< previous page
page_xiii
next page >
Page xiii Foreword The preparation of inorganic materials by thermolysis of preceramic compounds has become of substantial interest for the production of innovative materials in recent years. The general idea of this type of process route is that element-organic precursor molecules are constituted of structural units of the inorganic material aimed for by this process, thus providing novel paths of controlling the atomic array, composition and microstructure of materials. Of special interest is the manufacture of amorphous or nano-crystalline covalently bounded inorganics on the basis of silicon, boron, carbon and nitrogen, revealing a unique potential of properties not known from conventionally prepared materials. It is the intention of this book to provide a comprehensive survey on the French contributions to the synthesis of nano-sized powders and the production of nano-structured silicon-based composites by liquidphase sintering using nano-sized powders where interfaces play a decisive role for the evolution of properties. The infrared laser thermolysis of gaseous or liquid precursors is a highly versatile method well-fitted for the production of silicon-based amorphous or crystalline nanopowders. Due to the purity level and degree of dispersion, such powders are good candidates for the application in ceramics. Apart from ‘pure’ powders consisting of silicon, carbon and/or nitrogen, such ones containing homogeneously distributed alumina and yttria are typically used as sintering aids for silicon carbide and silicon nitride based materials. It has been proven that there is a strong influence of the carrier gases used for the synthesis laser process on residual hydrogen bonded to silicon, carbon and/or nitrogen providing some functionality during further thermal treatments. For the analysis of the amorphous and nano-crystalline structure of the as-thermolysed and heat treated powders, morphological and analytical transmission electron microscopy studies are decisive. Chemical ordering of the material such as powders in particular is analysed by nuclear magnetic resonance studies. Further analytical investigations are electron paramagnetic resonance, X-ray photoelectron spectroscopy, Xray absorption spectroscopy, X-ray and neutron diffraction. Furthermore, numerical simulations are used for the study of the chemical disorder and to propose structural models for the structure of the amorphous state of the materials. The content of the book is – even though very comprehensive – very detailed and strongly interdisciplinary. Therefore, the book is valuable for a broad readership in research and education.
< previous page
page_xiii
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_xiii.html [20/01/2010 10:03:01 AM]
page_xiv
< previous page
page_xiv
next page >
Page xiv The editors are well-known experts in the field of research covered by the book. They can be congratulated for a proper selection of authors and for providing an excellent piece of work. Fritz Aldinger Max-Planck-Institut für Metallforschung, Stuttgart, Germany June 2001
< previous page
page_xiv
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_xiv.html [20/01/2010 10:03:01 AM]
page_xv
< previous page
page_xv
next page >
Page xv Preface Physical properties of solids are greatly influenced by the arrangements of atoms present in the network. Nanostructured systems can offer improved and new properties compared to those of bulk materials. Consequently, in such materials, the influence of interfaces and interphases are of noticeable importance. Such interactions between the grains can lead to new physical and chemical properties. In recent years, an increasing interest has been devoted to nanostructured composites. This attention is largely due to exciting possible applications ranging from new catalysts to the preparation of nanocomposite ceramics, with significant improvements in their properties. Ceramic composites, obtained by dispersing nanoscale particles of one constituent into larger particles of a second constituent, have shown such improvements in mechanical properties (micro/nano composites). In particular, superplasticity has been obtained by mixing two equally fine constituents (nano/nano composites). Different modes of preparation have been used to make nanosized particles in large enough quantities. Among them, laser ablation of solid targets, plasma- or laser-induced reactions of gaseous mixtures have been developed. Other methods are related to evaporation– condensation, ball milling, self-propagating high temperature synthesis, sol–gel, spray drying of solutions, aerosol pyrolysis and chemical vapour decomposition at low pressure. Due to the large variety of such materials, comparative analysis is questionable. The originality of the book consists principally of focusing on a series of identical materials including preparation conditions, physical and chemical analysis, preparation and mechanical property determination of silicon-based nanocomposites. André P. Legrand (
[email protected])
< previous page
page_xv
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_xv.html [20/01/2010 10:03:02 AM]
page_xvi
< previous page
page_xvi
next page >
Page xvi Acknowledgements We thank the Chemistry Department of the Centre National de la Recherche Scientifique (CNRS), which endorsed this work through a Groupe de Recherche (CNRS GdR 1168), for its interest and partial support, and more particularly its Director Jean-Claude Bernier and Associate Director Pierre Henri Dixneuf. The Délégation Générale pour l’Armement contributed to the development of this research through its financial support. We express here our sincere thanks.
< previous page
page_xvi
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_xvi.html [20/01/2010 10:03:02 AM]
page_1
< previous page
page_1
next page >
Page 1 1 Objectives and state-of-the-art of nanocomposites Michel Cauchetier and André Pierre Legrand 1.1 Introduction Processes to make new ceramic materials are many and depend on the final desirable structure and macroscopic shape to be obtained. So silicon carbide can be used as an abrasive, refractory, structural material or semiconductor with a negative temperature coefficient. Processes developed to produce such materials are extremely diversified. A process is selected based on the required properties and structural shape of the parts to be obtained. As an example, the preparation of carbon fibres, which needs specific polymer precursors for spinning followed by heat and oxidation treatments, had been adapted to the preparation of silicon carbide fibres. Other processes of transformation, descended from physics or chemistry domains are chemical vapour deposition, chemical liquid deposition, etc. (Figure 1.1). They are able to present improved mechanical, thermal or electrical properties, not solely depending on a peculiar chemical composition but on the arrangement of the crystalline phases or the size of the grains. Nanocomposites constitute a new class of extremely diversified materials which have appeared in the last decade.
Figure 1.1 Schematic representation of ceramic preparation showing the feedback process leading to a new ceramic material involving three main steps: synthesis of a precursor; analytical methods; and sintering and validation of the physical and chemical properties.
< previous page
page_1
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_1.html [20/01/2010 10:03:03 AM]
page_2
< previous page
page_2
next page >
Page 2
Figure 1.2 Ceramic/ceramic micro–nano and nano–nano composites’ aspects (from Figures 7.8 and 7.20(b)). Sajgalik et al. (1996) proposed a classification into two main systems: • micro–nano composites in which the matrix is constituted by micrometric crystals embedded into a nanometric phase. Moreover, Niihara (1991) distinguishes three different configurations: intragranular, intergranular, intra/intergranular (Figure 1.2); • nano–nano composites in which the nanometric grains of the matrix and the second phase are spread uniformly (Figure 1.2). What makes a nanocomposite especially interesting is that at least one of its phases has dimensions in the nanometer range (10–100 nm). In this range, chemical and physical interactions have critical length scales and, if the nanoscale building block is made smaller than this one, the corresponding fundamental properties can be to changed. An example of this is light scattering, where by controlling the size of pores and nanocrystals in the range of 8 nm, Nanophase Technologies Corporation was able to produce transparent ceramics in the visible domain. Other enhanced properties have been developed (superplasticity, magnetoresistance, low temperature densification, enhanced and finer homogeneity, etc.). 1.2 Nanostructured ceramic elaboration Two main routes are generally used, depending on the densification rate and the properties to be obtained. 1.2.1 Amorphous ceramics obtained by solid state thermolysis of polymer precursors Pyrolysis, under a controlled atmosphere, of polymers, such as polysilazane, polycarbosilane, etc. is an efficient process for preparation of ceramics. According to Bill et al. (1999) ‘The in-situ crystallisation of these materials permits the preparation of nanocrystalline materials by a completely powder-free process. The structure and composition of the grain boundaries that originate from these crystallisation processes strongly depend on the molecular structure
< previous page
page_2
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_2.html [20/01/2010 10:03:03 AM]
page_3
< previous page
page_3
next page >
Page 3 of the initially used precursors.’ Such processes are particularly interesting in the preparation of fibres. 1.2.2 The powder-making processes To obtain nanocomposites it is necessary to prepare nanopowders so as to increase the reactivity of the different phases during the sintering process. This is due to a high surface/volume ratio (generally diameter < 100 nm). To obtain such powders, which have to present ideal characteristics (nanometric in size, spherical in shape, monodisperse, low agglomerated, high or controlled purity), it is necessary to develop new processes. These new methods must be innovative and need to be adapted to industrial production. Such recently developed processes deal with reactions such as • Solid phase: Evaporation–condensation, laser ablation, ball milling (or mechanical alloying), selfpropagating high-temperature synthesis (SHS); • Liquid phase: Sol–gel, spray-drying of solutions, aerosol pyrolysis; • Gaseous phase: Chemical vapour condensation at low pressure, plasma and laser synthesis. Some nanosized powders are now commercially available in the USA and in Japan: • Nanophase Technologies Corp. has developed a gas condensation process to produce different oxide powders (aluminium, titanium, zirconium oxides). • Nanodyne is focused on the production of cobalt–tungsten carbide, a ceramic–metal nanocomposite used to make tools for cutting and wear-resistant devices. • Ultram International produces ceramic and composite powders by a super-high-frequency plasma chemical process. • MarkeTech International proposes nanosized silicon carbide, silicon nitride, silicon carbonitride, boron carbide and silica powders obtained by a CO2-laser pyrolysis process. • Mitsubishi Mining & Cement Co. Ltd has prepared silicon/carbon/nitrogen nanocomposite powders from pyrolysis in a furnace of an organosilicon compound. A second problem which needs to be solved concerns the sintering for the preparation of complex shaped components so as to keep the initial size of the crystals. Similarly, the identification of the most efficient methods of characterisation, all along the different steps of preparation, is of significant importance. 1.3 Nanostructured Si3N4/SiC materials Different methods have been developed for the preparation of Si3N4/SiC nanocomposites by hot pressing sintering using: • Micrometric silicon nitride, previously recovered with carbon, so as to produce the carboreduction of silicon oxide present at the surface of the initial material: (Ishizaki and Yanai 1995; Watari 1989; Bahloul et al. 1993).
< previous page
page_3
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_3.html [20/01/2010 10:03:04 AM]
page_4
< previous page
page_4
next page >
Page 4 • Micrometric silicon nitride with nanometric Si/C/N or Si/C powders and sintering additives (Al2O3, Y2O3) (Niihara 1990). Nevertheless, the mixture, in a liquid medium, of such different sized powders containing so many different chemical groups on the surface, is difficult to obtain. This produces agglomerates and a heterogeneous distribution of the second phase in the matrix. • Nanometric Si/C/N or Si/C powders with sintering additives (Al2O3, Y 2O3) (Sasaki 1993; Kaiser 1996; Kennedy 1996). 1.4 Analytical methods Different methods can be used for the characterisation of initial to heat-treated and/or pressurised precursors such as: • Chemical analysis (CA) • Electron paramagnetic resonance (EPR) • Extended X-ray absorption fine structure (EXAFS) • Infrared spectroscopy (IR) • Soft X-ray spectroscopy (SXS) • Solid state nuclear magnetic resonance (NMR) • Specific surface area determination (SA) • Transmission electron microscopy and electron diffraction (TEM) • X-ray (XD) and neutron (ND) diffraction • X-ray photoelectron spectroscopy (XPS). Such methods are able to provide information of varied nature, depending on the origins of the physical phenomena involved (Table 1.1). Another important remark concerns the method of preparation of the sample. From the as-formed, heat treated and sintered sample, it is necessary to arrive at a condition adapted to the method of measurement. Crushing the material and filling, dispersing, spreading it in/on the sample holder are able to influence the results. This is why cross measurements are necessary. Table 1.1 Available information depending on the method used Method Surface Bulk Crystalline Amorphous Local or short order Average or long order Sample type CA × × Powder EPR × × Powder EXAFS × × × Powder IR × × × Powder ND × × × Powder NMR × × × × × Powder SXS × × Any TEM × × × Nanopowder XD × × × Powder XPS × × × × Any SA × × Any Note × Indicates the dominant domain of expertise of the method.
< previous page
page_4
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_4.html [20/01/2010 10:03:04 AM]
page_5
< previous page
page_5
next page >
Page 5 Some examples shown in this book demonstrate such phenomena: • X-ray, TEM and NMR. Figure 2.3, section on Si/C-based powders in Chapter 4 and Figure 5.1.6: α-β-SiC and amorphous detected in different proportions; • NMR and TEM. Figures 4.65, 4.66 and 5.1.27: Si3N4 detected in the bulk and not into grains; • XPS and NMR. Figures 5.3.10 and 5.1.10: SiO2 detected on the surface and not in the bulk; where the different phases are not evaluated with the same efficiency. 1.5 Conclusion Although till now many studies on that subject have been published, results are contradictory and fragmentary. No interdisciplinary studies, till now, have been done on the silicon nitride– silicon carbide system. A better knowledge of the behaviour and potential of such materials is needed. Elaboration of high-temperature ductile nanocomposites is one of the objectives of this work. Consequently, systematic studies and analyses of the preparation proceed from step by step. Chemical bonding, nanostructure, microstructure and monolith material properties are determined. Such an approach allows us to obtain original results for each step of the preparation and to establish relations between the synthesis of powders, their sintering aptitude, the development of the microstructure and the properties obtained. The spiral in Figure 1.1 represents this symbolically. References Bahloul, D., Pereira, M. and Goursat, P. (1993) J. Am. Ceram. Soc., 76(5), 1156–68. Bill, J., Wakai, F. and Aldinger, F. (1999) Precursor-Derived Ceramics. Wiley-VCH. Ishizaki, K. and Yanai, T. (1995) Silic. Indus., 7–8, 215. Kaiser, A. (1996) Silic. Indus., 5–6, 215. Kennedy, T. (1996) Silic. Indus., 9–10, 201. Niihara, K. (1990) J. Mater. Sci. Lett., 10, 112. Niihara, K. (1991) The Centennial Memorial Issue of the Ceramic Society of Japan, 99(10), 974. Sajgalik, P., Dusza, J., Hofer, F., Warbichler, P., Reece, M., Boden, G. and Kozankova, J. (1996) J. Mater. Sci. Lett., 15, 72. Sasaki, G. (1993) Mater. Res. Soc. Symp., 287, 335. Watari, K. (1989) Mater. Sci. Eng., A109, 89.
< previous page
page_5
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_5.html [20/01/2010 10:03:05 AM]
page_6
< previous page
page_6
next page >
Page 6 2 Laser synthesis of nanosized powders Michel Cauchetier, Emmanuel Musset, Michel Luce, Nathalie Herlin, Xavier Armand and Martine Mayne 2.1 Generalities on the synthesis of nanosized powders by laser pyrolysis 2.1.1 The laser pyrolysis process Infrared laser pyrolysis (IRLP) is a highly versatile method for the production of a wide range of nanopowders including SiC, SiCN, SiCO, BN and carbon (Haggerty and Cannon 1981; Cauchetier et al. 1988, 1994; Herlin et al. 1996; Boulanger et al. 1995; Ehbrecht et al. 1993; Voicu et al. 1996). A summary of the syntheses performed so far for materials applications is given in Table 2.1 and completes the review appearing in Knudsen (1997). In the IRLP process, the reactants are heated by IR laser radiation and decompose, causing clusters to nucleate and grow rapidly. This process is inherently very clean because homogeneous nucleation occurs in a well-defined reaction zone without interaction with chamber walls. The small reaction volume and the ability to maintain steep temperature gradients (106 °C/s) allow precise control of the nucleation rate, growth rate and residence times. The physical and chemical properties of the particles can be controlled by changing the molecular precursors and the synthesis parameters (laser power, pressure, etc.). The resulting powders are very fine, spherical, extremely pure, more or less agglomerated and nearly monodispersed in size. The mean particle size can be adjusted from 10 to 100 nm. All these characteristics (i.e. nanometric size (<100 nm) spherical shape, narrow size distribution, limited agglomeration and high purity) make laser powders good candidates for use in ceramics. 2.1.2 Developments and economic analysis Since the synthesis of Si and Si3N4 (Haggerty and Cannon 1981), the production of ultrafine powders from gaseous reactants has become an innovative application of lasers in chemistry. Although the CO2 laser synthesis of powders for use in ceramics is a new process compared with plasma or sol–gel processes, it offers considerable promise and it has been developed in several countries: in Europa (France at the CEA, Italy at the ENEA and the CISE, The Netherlands at the TU Delft, Germany in Jülich), in Japan and China. The laser synthesis technique requires the presence of a species which absorbs laser radiation such as SiH4. This precursor has been widely used to obtain silicon-based ceramic powders (see Table 2.1 and references therein). Production rates at laboratory scale have reached 100 g/h or more for silicon carbide (Cauchetier et al. 1988) and the development of the process for a pilot can be estimated to require a production rate of 1– 10 kg/day (Garifo 1995). Recent economic considerations have shown that SiH4 which is only available as
< previous page
page_6
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_6.html [20/01/2010 10:03:05 AM]
page_7
< previous page
page_7
next page >
Page 7 Table 2.1 CO2 laser synthesized nanometric powders Powders Chemical Si SiH4
systems References Haggerty and Cannon 1981; Cauchetier et al. 1987 SiC SiH4 + C2H4 Sumaya et al. 1985; Cauchetier et al. 1987; Förster et al. 1991 SiH4 + C2H2 Cauchetier et al. 1987; Curcio et al. 1989; Fantoni et al. 1990; Tougne et al. 1993 SiH4 + CxHy with x = 4 Cauchetier et al. 1988 SiH2Cl2 + C2H4 Suzuki et al. 1992 (CH3)2Si(C2H5O)2 vapour Li et al. 1994a Si3N4 SiH4 + NH3 Haggerty and Cannon 1981; Kizaki et al. 1985; Symons and Danforth 1987; Buerki et al. 1990 SiH2Cl2 + NH3 Bauer et al. 1989 SiC + Si3N4 or Si/C/N [(CH3)3Si]2NH vapour Rice 1986; Li et al. 1994b SiH4 + CH3NH2 + NH3 Cauchetier et al. 1989; Cauchetier et al. 1991 SiH4 + (CH3)2NH + NH3 Alexandrescu et al. 1991; Borsella et al. 1992 SiH4 + C2H4 + NH3 Suzuki et al. 1993 (CH3SiHNH)x with x = 3 or 4 (aerosol) Gonsalves et al. 1992 [(CH3)3Si]2NH (aerosol) Cauchetier et al. 1994; Herlin et al. 1994; Musset et al. 1997 SiO2 Si(C2H5O)4 (aerosol) Luce et al. 1994 SiO2 + SiC + C or Si/C/ (RO)4−xSi(R′)x with 0 = x = 3, R = Armand et al. 1995; Martinengo et al. O C2H5O, R′ = CH3 and [(CH3)3Si]2O 1996; Herlin et al. 1996; Fusil et al. 1997 (aerosol) BN BCl3 + NH3 Luce et al. 1993; Baraton et al. 1994; Willaime et al. 1995 B4C BCl3 + CH4 + H2 Knudsen 1987a BCl3 + C2H2 + H2 Luce et al. 1993 TiB2 TiCl4 + B2H6 Casey and Haggerty 1987a TiCl4 + BCl3 + H2 Knudsen 1987b ZrB2 Zr(BH4)4 Cauchetier et al. 1987; Rice and Woodin 1988 TiO2 Ti[OCH(CH3)2]4 Casey and Haggerty 1987b; Rice 1987; Curcio et al. 1991 TiC TiCl4 + C2H4 Alexandrescu et al. 1997 Al2O3 Al(CH3)3 + N2O + C2H4 Borsella et al. 1993 WC WF6 + C2H2 + H2 + SF6 Bourgeois et al. 1995 electronic grade remains too expensive (Cauchetier et al. 1994) for use in large quantities (>1 ton/year) even if energy and laser equipment costs are low compared to the raw material costs. In the case of Si3N4 laser synthesis, a study of the economics shows that a price for SiH4 less than one-fourth of its current price is needed to compete with a classic method of synthesis (Schoenung 1991). Alternative methods have been proposed with the substitution
< previous page
page_7
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_7.html [20/01/2010 10:03:06 AM]
page_8
< previous page
page_8
next page >
Page 8 of chlorosilanes (Bauer et al. 1989; Suzuki et al. 1992) or organosilicon compounds (Rice 1986; Gonsalves et al. 1992; Cauchetier et al. 1994) for silane. Technical improvements in two different fields have enhanced the versatility of the method. First, new introduction systems for the silicon (Si) precursors have been tested. Liquid organosilicon compounds are introduced into the laser beam in the aerosol form, fine liquid droplets being obtained by ultrasonic nebulisation (Gonsalves et al. 1992; Cauchetier et al. 1994). Second, the use of high-power tunable continuous wave (c.w.) CO2 lasers, now available, has increased the area of applications of the process (Luce et al. 1994). In this chapter, the synthesis of Si-based powders by two methods, using gaseous or liquid precursors, will be presented: • SiH4 as gaseous precursor for the synthesis of Si, SiC, Si3N4 and SiC–Si3N4 mixture powders and also methylsilane, SiH3CH3, for the synthesis of SiC powder, • hexamethyldisilazane [(CH3)3Si]2NH or HMDS as liquid precursor for the synthesis of Si/C/N (silicon carbonitride) powders; mixture of organosilicon precursors for the synthesis of Si/C/N powders containing the elements of sintering additives. 2.2 Synthesis of Si, SiC, Si3N4 and SiC Si3N4 mixtures with SiH4 and SiH3CH3 as silicon precursors 2.2.1 Experimental setup The experimental device is presented in Figure 2.1 (Cauchetier et al. 1991). The unfocused Gaussian beam (diameter = 12 mm) of a high-power c.w. CO2 laser (CILASCI1000, Marcoussis, France) enters the reaction cell through a KCl window and crosses the path of the gaseous flow of the reactants injected through an inlet capillary (inner diameter = 2mm).
Figure 2.1 Schematic laser irradiation cell for gaseous precursors. (Reprinted from Cauchetier, M., Croix, O., Luce, M., Baraton, M. I., Merle, T. and Quintard, P., (1991) Journal of the European Ceramic Society, Nanometric Si/C/N Composite Powder: Laser Synthesis and IR Characterisation, 8, 215, with permission from Elsevier Science.)
< previous page
page_8
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_8.html [20/01/2010 10:03:06 AM]
page_9
< previous page
page_9
next page >
Page 9 A resonance effect between the emission line of the laser at 10.6 μm and an infrared absorption band of one of the reactant gases (silane, SiH4 or methylsilane, CH3SiH3) causes the reaction to occur. This laser-driven reaction leads to high temperatures (up to 1800°C) and a bright flame. An argon flow prevents powder deposition on the windows and guides the products into the collection chamber. The powders are collected and then stored in a glove-box under argon atmosphere to avoid contamination by air or water vapour. 2.2.2 Synthesis results Table 2.2 summarises the synthesis conditions of the different powder samples used in different parts of this book (Si, SiC, Si3N4 and mixtures of SiC/Si3N4) and also presents first characterisation results. For all the experiments reported here, the cell pressure was kept constant at 1 atmosphere (105 Pa). In Table 2.2, most of the results concern SiC and Si/C/N synthesis, but some results shows the synthesis of Si from pure SiH4 (Si50), Si3N4 from a mixture of SiH4 and NH3 (SiN7). Structural investigations on both these powders are presented in Chapter 5. SiC powders have been obtained from methylsilane (SiC151, SiC152) or from mixtures of SiH4 and C2H2. In the run, SiC171 diborane was added in the silane/acetylene mixture, as a boron source used for sintering aid in densification tests (Croix et al. 1991), and after pressureless sintering at 2000°C, densities up to 0.95 were achieved. The last samples presented in Table 2.2 are Si/C/N samples, obtained from a mixture of SiH4, CH3NH2, and, in some cases, NH3 has been added to the reactive mixture. In two runs (Si50, SiC163), an inert gas (Ar, He) has been added to the reactive gases in order to increase the linear velocity. After comparing the chemical composition of the gas phase with the chemical composition of the powder, the C/Si and C/N ratios were obtained (see Table 2.2). In some cases, the flame temperature was measured using an optical pyrometer. Specific surface area (S)was determined from Brunauer–Emmet– Teller (BET) measurements and the equivalent diameter (D) was calculated from these measurements. The time of residence in the laser beam is calculated from the gas flow rates (2 mm nozzle diameter, 12 mm laser beam diameter) assuming room temperature. From the results presented in Table 2.2, some information can be obtained on the effect of experimental parameters. Laser power Increasing the laser power, and keeping all the other parameters constant, leads to an increase in temperature, which is expected to have an influence on the powders produced. In experiments SiC151 and SiC152, the laser power has been decreased by a factor of three (600/220 W) and the measured temperature decreases from 1530°C to 1150°C. The same crystalline structure is identified by X-ray diffraction (XRD). Therefore, in this temperature range, the flame temperature does not influence the structure of the powder. In contrast, BET measurements indicate a decrease in the powder size as the temperature decreases. Thus, the temperature has a direct influence on the kinetics of the powder growth. Flow rates In runs SiC163–177, the flow rates have been changed keeping the laser power constant. Increasing the flow rates leads to a decrease in the residence time as shown in Table 2.2. Figure 2.2 presents the variation in the particle size of SiC powders with the residence time for samples SiC163–177. Figure 2.2 also presents results (broken line) obtained five years before
< previous page
page_9
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_9.html [20/01/2010 10:03:07 AM]
page_10
< previous page
page_10
next page >
Page 10 Table 2.2 Gas phase synthesis conditions and characterisation results of the different samples Samples Flow rates (cm3/min) Atomic Laser Temperature (° Residence BET XRD ratio (gas power C) time (ms) results phase) (W) SiH4 C2H2 He, CH3NH2NH3 C/N C/Si S D Ar (m2/ (nm) g) Si50 120 0 480 0 0 600 930 4.3 29 89 Si (Ar) SiC151 CH3SiH3 : 600 1530 13.0 34 55 β-SiC 200 SiC152 CH3SiH3 : 220 1150 13.0 52 36 β-SiC 200 SiC163 540 300 1000 0 0 1.1 600 1.2 117 16 (He) SiC171a 1080 600 0 0 0 1.1 600 1.3 135 14 SiC173 200 110 0 0 0 1.1 600 7.3 61 31 SiC174 350 192 0 0 0 1.1 600 4.2 74 25 SiC177 120 66 0 0 0 1.1 600 12.1 36 52 SiC212 596 306 0 0 0 1.0 640 2.5 70 27 SiN7 120 0 0 0 480 600 1250 4.3 71 26 SiCN12 340 0 0 200 0 600 1550 4.8 47 40 α, βSi3N4, β-SiC SiCN27 280 0 0 70 250 600 1615 4.3 26 72 α, βSi3N4 SiCN29 360 0 0 90 320 0.22 0.25 400 2.9 40 49 SiCN35 350 0 0 200 0 1 0.57 600 4.1 48 39 Note a 40 cm3 /min of diborane B2H6 added as boron source which acts as sintering aid for the densification of SiC.
< previous page
page_10
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_10.html [20/01/2010 10:03:07 AM]
page_11
< previous page
page_11
next page >
Page 11
Figure 2.2 SiC particle size v. the residence time in the laser beam (laser power, 600 W; cell pressure, 1 atm). Similar results have already been observed previously (– – –) with a laser power of 640 W. (Reprinted from Tougne et al. (1993) Diamond and Related Materials, Evolution of the Structure of Ultrafine SiC-Laserformed Powders with Synthesis Conditions, 2, 486–490, with permission from Elsevier Science.) the present results, with a higher laser power (640 W) (Tougne et al. 1993). It must be noted that the value obtained for the SiC212 (640 W) experiment (not plotted) is in good agreement with these early results. Figure 2.2 clearly shows a linear decrease in the size of the particles as the residence time decreases. Figure 2.3 presents the XRD diagrams of the SiC163–177 samples. The lines become sharper and the full width at half maximum (FWHM) decreases as residence time increases, which indicates an increasing size of crystallites, parallel to the increasing particle size (BET measurements). TEM observations also confirm the BET and XRD results. Sample SiC163 (Figure 2.4(a)) presents fine spherical particles with a mean diameter of 20 nm (BET measurement: 16 nm) and with a unimodal distribution. They are not fully crystallised and appear as fine crystallites in an amorphous matrix. It clearly shows that the size of the particles (BET) and the size of the crystallites (XRD) must be distinguished. Sample SiC177 (Figure 2.4(b)) also presents fine spherical particles with an increased mean diameter of 60 nm (BET measurement: 52 nm). They are well crystallised with some black streaks. In correlation with the chemical composition C/Si = 1.1, some fine filaments of turbostratic carbon (C) can be noticed. In conclusion, it must be noted that both laser power and flow rates have a noticeable effect on the size of the particles. A good control of these experimental parameters allows a good control of the size and the structure of powders. Some other points which are relevant for materials applications must be noted: • The amount of synthesised powders is significant. For example, in the run SiC171, a production rate of about 100 g/h indicates that the process can be easily scalable. The
< previous page
page_11
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_11.html [20/01/2010 10:03:08 AM]
page_12
< previous page
page_12
next page >
Page 12
Figure 2.3 XRD patterns of the as-synthesised SiC powders (arbitrary units (a.u.)). (Reprinted from Tougne et al. (1993) Diamond and Related Materials, Evolution of the Structure of Ultrafine SiC-Laser-formed Powders with Synthesis Conditions, 2, 486–490, with permission from Elsevier Science.) duration of the experiment can be 3 h or more in order to collect powder quantities in the 150–200 g range for the elaboration of materials. • Also, a very good reproducibility of the experiments can be achieved; for example, Table 2.2 shows BET results for the runs SiCN12 and SiCN35 undertaken after a delay of 4 years. • Another interesting point is the good yield of the reaction. For example, in the SiC212 run, and supposing 100% conversion of SiH4 and C2H2 to the solid phase, the maximum calculated production rate is 64 g of SiC per hour and the experimental result is 59 g/h – this reaction yield (almost 100%) is very good. 2.2.3 Chemical analyses of the as-formed powders The chemical composition in stoichiometric compounds (Si3N4, SiC, SiO2, Si, C) has been calculated from elemental analysis results, with the classical assumption that all O is in the form of SiO2, then all N forms Si3N4 and the remaining Si is in the form of SiC. Free C (or Si) is the difference between total C (or Si) and C (or Si) bonded to Si (or C) in SiC. Such a calculation is useful to evaluate the composition of future sintered materials, or to compare several powders but it is obvious that it is only an approximation, especially when the powders are not fully crystallised.
< previous page
page_12
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_12.html [20/01/2010 10:03:08 AM]
page_13
< previous page
page_13
next page >
Page 13
Figure 2.4 TEMs of two as-formed powders: (a) SiC163; (b) SiC177. SiC powders In order to avoid the presence of free Si in the powders which makes the powder very sensitive to oxygen contamination, most of the SiC samples were synthesised with a gaseous mixture containing excess C (C/Si = 1.1 in the gaseous mixture). In Table 2.3, two examples show that this ratio is also found in the powders produced. In agreement with the chemical composition, XRD patterns (similar to Figure 2.3) correspond to the β-SiC phase. The O and free C contents are low and correspond to the values usually encountered for commercial powders. Table 2.3 also presents the chemical composition calculated in stoichiometric compounds which indicates, in good agreement with the XRD pattern, that the powders are mostly composed of SiC. Si/C/N powders For the synthesis of Si/C/N composite powders, two gaseous mixtures were investigated: a binary mixture SiH4 + CH3NH2 (SiCN35) and a ternary mixture: SiH4 + CH3NH2 + NH3
< previous page
page_13
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_13.html [20/01/2010 10:03:09 AM]
page_14
< previous page Page 14 Table 2.3 Chemical characterisations of gas Powder Samples Chemical analysis (wt%) Si C N SiC173 68.3 30.2 0 SiC212 68.3 30.3 0 SiCN29 58.3 6.5 34.6 SiCN35 66.9 13.6 18.2
page_14
next page >
phase synthesised powders
Atomic ratio Chemical composition (wt%) O C/Si C/N Si3N4 SiO2 SiC 0.9 1.03 0 1.5 96 1.4 1.03 0 2.7 95.7 0.6 0.27 0.22 86.6 1.1 8.3 2.3 0.47 0.87 45.1 4.3 45.1
C 2.0 1.6 4.0 0
Si
0 0 0 5.5
Figure 2.5 XRD patterns of as-formed SiCN nanopowders used in material elaboration. (Reprinted from Mayne 1997.) (SiCN29) (Table 2.2). In the case of SiCN29, the presence of NH3 is known to make the nitriding introduce an increase in the nitrogen (N) content. For SiCN35 a similar content in C and N is expected in the resulting powder due to the C/N initial atomic ratio of 1 in the formula of monomethylamine. Tables 2.2 and 2.3 show a very good correlation between C/Si and C/N ratios in the gas phase and in the powder for SiCN29, but the correlation is not so good for SiCN35 probably due to evolution of carbonaceous gas of C in the gas phase during the synthesis. Chemical composition calculations show that the powder SiCN35, containing free Si is the most sensitive to oxygen contamination. XRD patterns (Mayne 1997) are reported in Figure 2.5 and confirm the calculated compositions. The SiCN29 sample contains mainly α- and β-Si3N4; the quantity of SiC is too small and is not detectable. The SiCN35 sample presents the characteristic lines of Si and β-SiC and a broad peak between 2θ = 30° and 40°, which can be attributed to an amorphous phase of silicon carbonitride. From the results presented in this section, it appears that the decomposition in stoichiometric compounds is a good representation of the powder and also that the chemical composition of the powders produced is most often well controlled by the chemical composition of the gaseous reactants. Together with the possibility of controlling the size and the structure of
< previous page
page_14
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_14.html [20/01/2010 10:03:10 AM]
page_15
< previous page
page_15
next page >
Page 15 the powder, it makes this synthesis technique attractive. But, as explained before, in order to increase the safety and decrease the cost, it has been applied to the liquid precursors containing Si, C and N elements. 2.3 Synthesis of silicon carbonitride (Si/C/N) powders using hexamethyldisilazane as Si precursor 2.3.1 Experimental Choice of the precursor As noted before, investigations based on costs of various silicon precursors for the delivery of large quantities have shown that silane remains too expensive for use in ceramic powder synthesis (Cauchetier et al. 1994). In our case [(CH3)3Si]2NH or HMDS with a Si cost very low compared to the Si cost of SiH4 (43 US$/kgSi in HMDS and 343 US$/kgSi in SiH4)was chosen as a model of the liquid precursor in order to demonstrate the possibility of using liquid wastes of the organosilicon compound chemistry for the synthesis of nanometric Sibased powders. Indeed, HMDS has a strong IR absorption band at 10.6 μm due to the Si N bond, which was, therefore selected. It is a common liquid Si compound (boiling point of 125°C, density of 0.76, and a viscosity of 0.69 cP at 25°C) largely used for the silylation of a wide range of functional groups and it was the precursor used by Niihara and co-workers in the synthesis of Si/C/N powders leading to non-oxide superplastic ceramics (Wakai et al. 1990). The first experiments using HMDS in the vapour phase as Si precursor for Si/C/N powder synthesis by CO2-laser pyrolysis were performed by Rice (1986). A conversion efficiency (liquid → powder) of about 60% has been obtained but with low flow rates of HMDS(7 g/h) and with a low-powered CO2 laser (135 W). Higher production rates have been attained (80–120 g/h) when the laser power has been increased to the 500–1000 W range (Li et al. 1994b). The experimental device The apparatus is shown in Figure 2.6. Liquid HMDS is placed in a special glass jar containing a piezoelectric transducer (Pyrosol 7901 type from RBI, Meylan, France, apparatus developed in collaboration with the CEA (Spitz and Viguié 1970)). The focusing of the intense beam of ultrasonic energy delivered by the transducer near the surface of the liquid yields uniform droplets whose diameter d is given by
where σ and ρ are the surface tension and the density of the liquid, respectively, and f the frequency of the transducer (here 850 kHz). In order to increase the mass of the displaced liquid, the glass jar is heated near 90–100°C with a heating ribbon. The aerosol droplets and vapour are injected into an irradiation cell very similar to those presented in Figure 2.1. The reaction cell is maintained at a regulated pressure of 105 Pa using a flow of argon or an argon–ammonia mixture through a glass inlet tubing (inner diameter of 13 mm). The laser beam diameter is increased from 12 to 24 mm with a beam expander in order to cover the reactant flow entirely. The initial laser power is in the range 480–520 W.
< previous page
page_15
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_15.html [20/01/2010 10:03:11 AM]
page_16
< previous page
page_16
next page >
Page 16
Figure 2.6 Schematic of the aerosol generator with the irradiation cell and the powder collector. 2.3.2 Synthesis results Table 2.4 compares the influence of two parameters, the nature of the carrier gas (argon and nitrogen) and heating of the liquid precursor (near 100°C), on the synthesis results. It can be seen immediately that the yield of the reaction (expressed as the ratio between the mass of powders produced and the mass of displaced liquid), does not appear to be as good as in the gas phase. Both the amount of displaced liquid and production rate increase when the precursor is heated. The effect of the heating is to combine the enrichment of the gaseous phase in HMDS vapour and decrease the viscosity of the liquid. In order to work with significant amounts of powders, most of the experiments were carried out with liquid heating. The yield seems independent of the heating of the precursor, but is strongly dependent on the nature of the gas. It is 46–49% for Ar carrier gas flow and 38–39% for N2 carrier gas flow.
< previous page
page_16
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_16.html [20/01/2010 10:03:11 AM]
page_17
< previous page
page_17
next page >
Page 17 2.3.3 Effect of experimental parameters Effect of carrier gas (Ar or N2) Table 2.4 shows that the chemical composition of the powder does not depend on the nature of the carrier gas flow (Ar or N2) and the C/N atomic ratio remains stable in the 2.5–2.9 range. The activity of atomic N (N2 ↔ 2N) is low at the measured flame temperature: 1260±20°C. Table 2.4 also shows that all powders are sensitive to pollution by oxygen, but the powders obtained from the heated precursor seem the most sensitive to pollution. It must be noted that the chemical analysis presented in this section is not complete due to the presence of hydrogen in the powder and due to the uncertainty of the measurements. Effect of chemical evolution of the reactive mixture Table 2.5 presents the synthesis parameters of all the samples studied in the different parts of this book. Only samples HMDS40–45 where the effect of chemical composition has been Table 2.4 Effect of the carrier gas nature and precursor heating Run Carrier gas Displaced Powder Yield SBET Chemical analysis (wt C/N flow rate (cm3/ liquid (cm3/h) production rate (wt%) (m2/g) %) (Atomic min) (g/h) ratio) Ar N2 Si C N O HMDS28a 2430 — 108 38 46 88 49.8 30.3 12.3 5.6 2.9 HMDS36b 2500 — 164 61 49 82 45.8 28.0 11.7 9.7 2.8 HMDS38b — 2500 166 48 38 125 47.2 28.4 12.8 11.6 2.6 HMDS39a — 2500 95 28 39 79 49.9 29.7 14.1 5.2 2.5 Notes a Liquid precursor at room temperature. b Liquid precursor heated near 100°C. Table 2.5 Synthesis conditions and chemical analysis of HMDS samples (chemical analyses were always performed after several weeks of exposure to air) Run Carrier gas flow rate Displaced Powder Yield SBET Chemical analysis (wt C/N (cm3/mn) liquid (cm3/ production (wt (m2/ %) (Atomic Ar N2 Total h) rate (g/h) %) g) Si C N O ratio) HMDS40 1935 205 2140 182 59 43 110 46.7 25.3 21.8 6.1 1.35 HMDS41 1770 410 2180 160 61 50 93 46.1 20.5 25.2 6.7 0.95 HMDS42 1570 600 2170 175 75 56 98 44.4 18.5 29.7 7.7 0.73 HMDS43 1370 800 2170 179 74 53 95 48.3 15.5 26.8 8.0 0.67 HMDS44 1150 1040 2190 210 81 51 95 47.1 13.1 26.7 10.9 0.57 HMDS45 830 1346 2180 167 66 52 106 47.6 8.3 28.9 13.4 0.34 HMDS35 1600 1000 2600 87 21 32 144 47.3 6.6 33.4 9.8 0.23 HMDS66 1920 1920 114 32 36 66 51.2 31.9 15.1 1.8 HMDS67a 1440 1920 115 31 35 66 52.0 30.8 14.8 2.4 HMDS73a 862 207 1920 56 14 32 115 51.9 12.6 25.3 10.1 Note a H2 in the carrier gas
< previous page
page_17
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_17.html [20/01/2010 10:03:12 AM]
page_18
< previous page
page_18
next page >
Page 18
Figure 2.7 C/N atomic ratio in as-formed HMDS powders v. C/N atomic ratio in the precursors (liquid + ammonia). (Reprinted from Musset et al. 1997 with the permission of the Belgian Ceramic Society, Mons, Belgium.) closely studied will be commented on in this section; the main part of the results appear in the PhD thesis of Emmanuel Musset (Musset 1995). For this set of six experiments, the liquid temperature is about 100°C, the total flow rate of the carrier gas mixture remains constant and the corresponding residence time of the precursor in the laser beam is about 0.1 ms. Table 2.5 shows the influence of the addition of ammonia in the argon used as carrier gas, namely, on the chemical composition of the resulting powders (samples HMDS40–45). Figure 2.7 shows a good correlation between the C/N ratio in the as-formed powder and in the reactive mixture; the C/N atomic ratio decreases from 1.35 to 0.36 when the ammonia volume ratio increases from 10% to 60%. This correlation confirms the possibility of controlling the chemical composition of the powders. Table 2.5 shows that the contamination by oxygen becomes more and more important when the N content in the powder increases, because NH bonds are easily hydrolysed. 2.3.4 First characterisations Specific surface area The specific surface area is always high, about 100 m2/g and taking into account the mean value of the density i.e. 2.00 (pycnometry measurement), the corresponding mean value for the diameter is 30 nm, in agreement with TEM observations.
< previous page
page_18
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_18.html [20/01/2010 10:03:12 AM]
page_19
< previous page
page_19
next page >
Page 19
Figure 2.8 IR spectra of the as-formed HMDS powders. (Reprinted from Musset 1995.) Infrared spectroscopy IR spectra of the samples HMDS40–45 are shown in Figure 2.8. They present a broad absorption band between 750 and 1250 cm−1 with a maximum at 920–940 cm−1 due to a Si/C/N amorphous phase, corresponding to a flat XRD diagram. A weak band at 550 cm−1 is due to the Si N bond. Other bands are related to hydrogenous species: N—H at 1180 cm−1, Si—H at 2050 cm−1 and Si—CH3 at 1250 cm−1, indicating an incomplete pyrolysis of the precursor or absorption of volatile species obtained from the pyrolysis. The presence of hydrogen is in good agreement with the chemical analysis, which is often less than 100% (Table 2.4). The results presented in this section show that it is possible to produce Si/C/N nanopowders with controlled chemical composition from a liquid precursor. The powders are obtained in significant quantities for materials applications. The main differences compared to powders obtained from the gas phase are the amorphous character and high hydrogen content of the powders obtained from the liquid phase. 2.4 Silicon carbonitride (Si/C/N) powders containing in situ the elements of the sintering aids (Al, Y): pre-mixed powders 2.4.1 Introduction: elaboration of SiC–Si3N4nanocomposite materials Materials in the SiC/Si3N4 system are elaborated by heat treatment of powders in the presence of liquidforming sintering aids such as Y2O3, MgO, Al2O3, etc. singly or in combination. Such processes need a previous mixing step of all powders having different natures and sometimes different sizes. Recently, some studies report the incorporation of metal elements
< previous page
page_19
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_19.html [20/01/2010 10:03:13 AM]
page_20
< previous page
page_20
next page >
Page 20 (Al, Y, etc.), necessary for the sintering step, into silicon nitride or carbonitride systems, most of them being focused on chemical processing routes using organometallic precursors (Soraru et al. 1992; Iwamoto et al. 1998; Koyama et al. 1998). A few other publications concern physico-chemical processes: laser irradiation of gaseous mixtures (SiH4, NH3, (CH3)3Al) allows the formation of nanosized powders with Al in a Si3N4 matrix (Borsella et al. 1993b). Aerosol of Si/C/N particles with yttrium and aluminium compounds were prepared under dual irradiation of CO2 and excimer laser beams of a SiH4, C2H4 and NH3 mixture, aluminium being incorporated in the form of alumina powder in the reactant flow and yttrium being introduced as a low volatile organometallic compound in the reaction zone (Yamada et al. 1997). 2.4.2 Synthesis of pre-mixed powders In order to prepare Si/C/N powders containing uniformly dispersed sintering aids investigations were undertaken to set up a laser spray synthesis process of Si/C/N/O/Al(Y) nanopowders using solutions of a liquid organosilicon precursor – HMDS – with solid metallic alcoxides, namely aluminium and yttrium isopropoxides [(CH3)2CHO]3Al and [(CH3)2CHO]3Y. Table 2.6 summarises the synthesis conditions of 14 runs which can be divided into 3 groups: • Group I includes experiments carried out with solutions having different Al (+Y)/Si atomic ratio. • Group II includes experiments carried out with solutions having the same Al (+Y)/Si atomic ratio. All runs are realised with a binary mixture of carrier gases (Ar + NH3). • The third is composed of experiments made with the same solutions as in group II, but the carrier gas is composed of Ar+NH3 +H2 in order to see if the chemical composition of the powders is modified by the presence of H2. Some changes occur compared to the experiments described above in Section 2.3. The initial laser power is in the range 300–330 W, but, here, with an unfocused laser beam (diameter = 13 mm) which covers the aerosol flow sufficiently. For comparison, an experiment with pure HMDS carried out under similar conditions is also reported (HMDS66). 2.4.3 Effect of experimental parameters Effect of the solutions of precursors In Table 2.6, most of the experiments were carried out with metallic isopropoxides in HMDS but, in two cases (HSAl04 and HSAlY05), isopropanol was added to the reactive solution in order to increase the solubility of the alcoxides and to decrease the viscosity of the solutions. In these experiments, more liquid is displaced than in other experiments but the production rate remains at the same level (≈30 g/h). Also, the amount of oxygen incorporated in the as-formed powders is very high (>10%). In conclusion, isopropanol does not improve the production or quality of the powders and this solution was not developed. Precursor solutions are characterised by their atomic ratios: [Al(+Y)]/Si. For the first experiments, the Al/Si ratio in the precursor solution was adjusted to 0.069 (e.g. HSAl03); this value corresponds to 6 wt% Al2O3 content in a final SiC/Si3N4 material according to the different oxide contents reported in the literature from about 10 (Kennedy et al. 1996) to 1 wt%
< previous page
page_20
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_20.html [20/01/2010 10:03:13 AM]
page_21
< previous page
page_21
next page >
Page 21 Table 2.6 Synthesis conditions and results of pre-mixed Si/C/N powders Run Carrier gas flow rates Displaced Powder SBET Chemicalanalysis (wt Atomic (cm3/min) liquid (g/h) production rate (m2/g) %) ratio Ar NH3 H2 (g/h) Si C N O Al Y Al + Y/ Al/ Si Y HSAl03 1900 0 0 87 34 6646.533.912.9 5.72.5 0 HSAl04 1900 0 0 119 32 8143.533.710.713.22.4 0 HSAl07 1900 0 0 88 24 11047.129.112.8 8.62.5 0 0.05 HSAl08 0 0 1900 49 11 28048.726.614.1 8.91.6 0 HSAlY05 1900 0 0 115 30 7943.733.411.211.51.71.4 HSAl09 1140 760 0 71 23 11249.5 6.836.0 6.11.5 0 0.03 HSAl12 1520 380 0 87 28 9647.214.829.0 7.51.5 0 0.03 HSAl13 1710 190 0 87 30 8349.823.019.2 5.92.0 0 0.04 HSAl11 475 570 855 64 27 13449.8 5.837.2 5.71.5 0 HSAl14 855 190 855 74 26 8948.817.324.5 7.71.6 0 HSAl15 665 380 855 75 22 9950.911.726.8 8.81.8 0 HSAlY16 1140 760 0 81 26 10053.0 7.530.3 8.20.40.4 0.01 3.0 HSAlY17 1520 380 0 89 25 9150.716.925.4 5.40.90.7 0.02 4.2 HSAlY18 1710 190 0 79 28 7749.321.922.4 5.10.50.7 0.01 2.5
< previous page
page_21
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_21.html [20/01/2010 10:03:14 AM]
page_22
< previous page
page_22
next page >
Page 22 alumina and yttria (Burger et al. 1997). The first result is that it is possible to incorporate Al and Y additives in the powders, but Table 2.6 clearly shows that the ratio Al/Si, in this range of experimental conditions, does not reach the 0.069 ratio. This is due to the preferential pulverisation of the most volatile compound of the mixture, that is, HMDS. So, in the following experiments, the initial Al/Si and (Al+Y)/Si ratios were decreased to 0.04 (HSAl09, 12, 13) and 0.02 respectively (HSAlY16, 17, 18). The similarity of the Al/Si atomic ratio in the starting solution (0.04) and in the as-formed HSAl powders (0.03–0.04) suggests that the nebulisation of the mixture of precursors is homogeneous. In the case of HSAlY powders, the Al/Y atomic ratios are different in as-formed powders (2.5–4.2) and in the starting solution (1.1), though (Al + Y)/Si atomic ratios remain similar (0.01– 0.02) to the starting solution. This is due to the incomplete dissolution of yttrium isopropoxide in HMDS and probably to an inhomogeneous nebulisation of the mixture of precursors. Effect of carrier gas The nature and composition of the carrier gas mixture play a significant role in the chemical composition of powders. Whatever the powder (HSAl or HSAlY), an increase of ammonia relative flow rate induces a decrease in C content and C/N atomic ratio as obtained for powders without sintering aids (Musset 1995). Table 2.6 also shows that when hydrogen is added partially in the place of argon in argon–ammonia mixtures, the C content decreases. This seems to indicate that more volatile hydrocarbon species are formed during the synthesis. For example, the C content varies from 14.8 to 11.7 wt% in a 80% argon–20% ammonia mixture (HSAl12 and 15 samples) and from 23.0 to 17.3 wt% in a 90% argon–10% ammonia mixture (HSAl13 and 14 samples). It must be noticed that a large quantity of free C (10–14%) remains in powders when the ammonia relative flow rate increases from 0 to 20. 2.4.4 First characterisations Specific surface area Powder production rates in the 22–34 g/h range and specific surface area values in 66–134 m2/g range are very similar to the values obtained for powders without metallic additives. Infrared spectroscopy and X-ray diffraction As for powders without metallic additives, XRD patterns show a large background without any distinct peak indicating an amorphous structure. This is confirmed by infrared spectra showing a large band around 900 cm −1. This one is essentially composed of Si—C bonds when powders are synthesised with argon-rich carrier gas while Si—N bonds in an amorphous environment (large band at 400 cm−1) appear with ammonia-rich carrier gas. Moreover, Si—CH3 bonds are present (1250 cm−1) in all powders. 2.5 Conclusion In this chapter, it has been shown that laser pyrolysis is a versatile method well suited for the production of significant amounts of Si-based nanopowders. Due to their properties (purity
< previous page
page_22
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_22.html [20/01/2010 10:03:14 AM]
page_23
< previous page
page_23
next page >
Page 23 limited only by the purity of the reactants, low size dispersion, etc.), the nanopowders are good candidates for applications in ceramics. Nanopowders can be obtained from gaseous or liquid precursors. The powders obtained from the gas phase are crystallised while the powders obtained from the liquid phase are amorphous. In both cases, the chemical composition of the powders is controlled by the chemical composition of the reactive mixture. Finally, an interesting result is the incorporation of the elements of sintering aids (Al, Y, O) during the synthesis. References Alexandrescu, R., Morjan, I., Borsella, E., Botti, S., Fantoni, R., Dikonimos-Makris, T., Giorgi, R. and Enzo, S. (1991) Journal of Materials Research, 6, 2442. Alexandrescu, R., Borsella, E., Botti, S., Cesile, M. C., Martelli, S., Giorgi, R., Turtu, S. and Zappa, G. (1997) Journal of Materials Science, 32, 5629. Armand, X., Herlin, N., Martinengo, H., Musset, E. and Cauchetier, M. (1995) Fourth Euro-Ceramics, vol. 1 (Faenza Editrice S.p.A., Faenza), pp. 37–44. Baraton, M. I., Boulanger, L., Cauchetier, M., Lorenzelli, V., Luce, M., Merle, T., Quintard, P. and Zhou, Y. H. (1994) Journal of the European Ceramic Society, 13, 371. Bauer, R. A., Smulders, R., Becht, J. M. B., Van der Put, P. J. and Schoonman, J. (1989) Journal of the American Ceramic Society, 72, 1301. Borsella, E., Botti, S., Fantoni, R., Alexandrescu, R., Morjan, I., Popescu, C., Dikonimos-Makris, T., Giorgi, R. and Enzo, S. (1992) Journal of Materials Research, 7, 2257. Borsella, E., Botti, S., Giorgi, R., Martelli, S., Turtu, S. and Zappa, G. (1993a) Applied Physics Letters, 63, 1345. Borsella, E., Botti, S., Alexandrescu, R., Morjan, I., Dikonimos-Makris, T., Giorgi, R. and Martelli, S. (1993b) Materials Science and Engineering A, 168, 177. Bourgeois, L., Barbier, G., Viguié, J. C., Herlin, N. and Cauchetier, M. (1995) Fourth Euro-Ceramics, vol. 1 (Faenza Editrice S.p.A., Faenza), pp. 225–232. Buerki, P. R., Troxler, T. and Leutwyler, S. (1990) High Temperature Science, 27, 323. Burger, P., Duclos, R. and Crampon, J. (1997) Materials Science and Engineering, A222, 175. Casey, J. D. and Haggerty, J. S. (1987a) Journal of Materials Science, 22, 737. Casey, J. D. and Haggerty, J. S. (1987b) Journal of Materials Science, 22, 4307. Cauchetier, M., Croix, O., Luce, M., Michon, M., Paris, J. and Tistchenko, S. (1987) Ceramics International, 13, 13. Cauchetier, M., Croix, O. and Luce, M. (1988) Advanced Ceramic Materials, 3, 548. Cauchetier, M., Croix, O., Robert, C., Lance, M. and Luce, M. (1989) Euro-Ceramics, vol. 1, Elsevier Applied Science, London, pp. 130–134. Cauchetier, M., Croix, O., Luce, M., Baraton, M. I., Merle, T. and Quintard, P. (1991) Journal of the European Ceramic Society, 8, 215. Cauchetier, M., Croix, O., Herlin, N. and Luce, M. (1994) Journal of the American Ceramic Society, 77, 993. Cauchetier, M., Armand, X., Herlin, N., Mayne, M., Fusil, S. and Lefevre, E. (1999) Journal of Materials Science, 34,1. Croix, O., Gounot, M., Bergez, P., Luce, M. and Cauchetier, M. (1991) Ceramics Today – Tomorrow’s Ceramics, Elsevier Science Publishers, Amsterdam, pp. 1447–1455. Curcio, F., Ghiglione, G., Musci, M. and Nanetti, C. (1989) Applied Surface Science, 36, 52. Curcio, F., Musci, M., Notaro, M. and Quattroni, G. (1991) Ceramics Today – Tomorrow’s Ceramics, Elsevier Science Publishers, Amsterdam, pp. 2569–2578. Fantoni, R., Borsella, E., Piccirillo, S., Ceccato, R. and Enzo, S. (1990) Journal of Materials Research, 5, 143. Förster, J., von Hoesslin, M., Schäfer, J. H., Uhlenbussch, J. and Viöl, W. (1991) Proceedings of the 10th International Symposium on Plasma Chemistry (FRG) vol. 1 (eds U. Ehlemann, H. G. Lergon and K. Wiesemann), pp. 1–6.
< previous page
page_23
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_23.html [20/01/2010 10:03:15 AM]
page_24
< previous page
page_24
next page >
Page 24 Fusil, S., Armand, X., Herlin, N. and Cauchetier, M. (1997) Key Engineering Materials, 132–136, 141. Garifo, L. (1995) Laser Focus World, 30. Gonsalves, K. E., Strutt, P. R., Xiao, T. D. and Klemens, P. G. (1992) Journal of Material Science, 27, 3231. Haggerty, J. S. and Cannon, R. W. (1981)Laser-induced Chemical Processing, Plenum Press, New York, pp. 165–241. Herlin, N., Musset, E., Luce, M. and Cauchetier, M. (1994) Journal of the European Ceramic Society, 13, 285. Herlin, N., Armand, X., Musset, E., Martinengo, H., Luce, M. and Cauchetier, M. (1996) Journal of the European Ceramic Society, 16, 1063. Iwamoto, Y., Kikuta, K. and Hirano, S. (1998) Journal of Materials Research, 13, 353. Kennedy, T., O’Neil, J. P., Hampshire, S., Poorteman, M. and Cambier, F. (1996) Silicates Industriels, 9–10, 201. Kizaki, Y., Kandori, T. and Fujitani, Y. (1985) Japan Journal of Applied Physics, 24, 800. Knudsen, A. K. (1987a) Advances in Ceramics, 21, 237. Knudsen, A. K. (1987b) US Patent 4, 689, 129. Knudsen, A. K. (1997) Carbide, Nitride and Boride Materials: Synthesis and Processing, Chapman & Hall, London, pp. 343–358. Koyama, S., Nakashima, H., Sugahara, Y. and Kuroda, K. (1998) Chemistry Letters, 191. Li, Y., Liang, Y., Zheng, F. and Hu, Z. (1994a) Journal of the American Ceramic Society, 77, 1662. Li, Y., Liang, Y., Zheng, F. and Hu, Z. (1994b) Materials Science and Engineering, A174, L23. Luce, M., Croix, O., Zhou, Y. H., Cauchetier, M., Sapin, M. and Boulanger L. (1993) Euro-ceramics II, vol. 1, Deutsche Keramische Gesellschaft, Köln, pp. 233–238. Luce, M., Herlin, N., Musset, E. and Cauchetier, M. (1994) Nanostructured Materials, 4, 403. Martinengo, H., Musset, E., Herlin, N., Armand, X., Luce, M. and Cauchetier, M. (1996) Silicates Industriels, 61,9. Mayne, Martine (May 1997) PhD Thesis, Limoges University, 97LIMO0021; http://thesenet.abes.fr Mayne, M., Armand, X., Cauchetier, M., Doucey, B., Bahloul-Hourlier, D. and Goursat, P. (1999) Ceramics: Getting in the 2000’s, Part B, Techna, Faenza, pp. 211–218. Musset, Emmanuel (Nov. 1995) PhD Thesis, Paris-Sud Orsay University, 95PA112537; http://thesenet.abes.fr Rice, R. W. (1986) Journal of the American Ceramic Society, 69, C183. Rice, R. W. (1987) Journal of the American Ceramic Society, 70, C117. Rice, R. W. and Woodin, R. L. (1988) Journal of the American Ceramic Society, 71, C181. Schoenung, J. M. (1991) American Ceramic Society Bulletin, 70, 112. Soraru, G. D., Ravagni, A., Dal Maschio, R. and Carturan, G. (1992) Journal of Materials Research, 7, 1266. Spitz, J. and Viguié, J. C. (1970) French Patent 2, 110, 622. Suzuki, M., Nakata, Y., Okutani, T. and Kato, A. (1992) Journal of Materials Science, 27, 6091. Suzuki, M., Maniette, Y., Nakata, Y. and Okutani, T. (1993) Journal of the American Ceramic Society, 76, 1195. Sumaya, Y., Marra, R. A., Haggerty, J. S. and Bowen, H. K. (1985) American Ceramic Society Bulletin, 1356. Symons, W. and Danforth, S. C. (1987) Advances in Ceramics, 21, 249. Tougne, P., Hommel, H., Legrand, A. P., Herlin, N., Luce, M. and Cauchetier, M. (1993) Diamond and Related Materials, 2, 486. Wakai, F., Kodama, Y., Sakaguchi, S., Murayama, N., Isaki, K. and Niihara, K. (1990) Nature, 344, 421. Willaime, F., Boulanger, L. and Cauchetier, M. (1995) Materials Research Symposium Proceedings, 359, 53. Yamada, T., Tanaka, Y., Suemasu, T. and Kohtoku, Y. (1997) Nuclear Instruments and Methods in Physics Research, B121, 378.
< previous page
page_24
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_24.html [20/01/2010 10:03:15 AM]
page_25
< previous page
page_25
next page >
Page 25 3 Thermal behaviour of as-formed silicon-based nanopowders General introduction This chapter presents the effects of thermal treatments on Si-based nanopowders obtained as described in the previous chapter from the gas phase or from the liquid phase. It is mainly focused on the behaviour of Si/ C/N and Si/C/N/Al/Y/O powders (0.2 < C/N(at) < 2.6) because such nanopowders may be used to obtain Si3N4/SiC materials after thermal treatment. This chapter is divided into two parts. The first part is devoted to thermal treatment in a high-temperature graphite furnace in order to know the evolution of the physico-chemical characteristics. The second part reports the study of the thermal behaviour using TGA/MS in order to determine the chemical reactions and mechanisms involved during annealing.
< previous page
page_25
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_25.html [20/01/2010 10:03:16 AM]
page_26
< previous page
page_26
next page >
Page 26 3.1 Thermal behaviour in a high-temperature graphite furnace Emmanuel Musset, Martine Mayne, Michel Cauchetier, Xavier Armand, Michel Luce and Nathalie Herlin-Boime 3.1.1 Introduction The aim of the first part of this study is to determine the influence of the annealing treatments performed in a high-temperature graphite furnace both on the weight of samples and on different physico-chemical properties of nanopowders such as the chemical composition, structure, reactivity and size. It is mainly focused on Si/C/N samples obtained from the liquid phase using the aerosol method. The results of annealing treatments and the consequences of these treatments on the chemical composition, size, organisation, etc. of silicon-based powders are presented with the intent of showing the similarities and the differences between the different powders, to correlate these properties to the synthesis conditions, etc., and to begin to compare the properties of these powders with the necessary properties for ceramic applications. 3.1.2 Weight evolution of SiC, Si/C/N and Si/C/N/Al/Y/O nanopowders The as-formed powders are annealed at atmospheric pressure in a high-temperature graphite furnace under argon or nitrogen (N) atmospheres. The temperature generally varies in the range 1000–1700°C, and the dwell time is 1 or 4 h. 3.1.2.1 Weight evolution under inert atmosphere Thermal treatments were performed on SiC or Si/C/N nanopowders in an argon atmosphere for temperatures up to 1600°C. SiC powders exhibit a weight loss whatever the temperature. The maximum weight loss, observed near 1500°C, remains low (usually <5 wt%) and is mainly related to the carboreduction of the silica by the free carbon (C), both present in the powders (1–3 wt%, Table 2.3) (Croix et al. 1991): (3.1.1) For Si/C/N powders obtained from the gas phase (SiCN29 and 35 in Table 2.2), a low weight loss (<10%) also occurs. This weight loss suggests a decomposition of the Si/C/N system. SiCN35 nanopowder exhibits a higher weight loss than SiCN29, which could be related to a stronger decomposition. It can also be partially explained by the carboreduction of silica, because of a higher amount of silica in the SiCN35 as-formed powder (Table 2.3). For Si/C/N nanopowders synthesised from HMDS, annealing experiments in argon at 1600°C lead to the formation of free silicon (Si) (Cauchetier et al. 1994) and the weight
< previous page
page_26
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_26.html [20/01/2010 10:03:16 AM]
page_27
< previous page
page_27
next page >
Page 27 loss is high (>20%). This also suggests the decomposition of the Si/C/N chemical system, which appears to be more important than in the case of Si/C/N obtained from the gas phase. Detailed mechanisms will be proposed and discussed in the TG–MS section. The decomposition of the Si/C/N chemical system under an inert atmosphere could be partially related to the degradation of the nitrogen-containing species inducing an evolution of nitrogen during the thermal treatment. Usually, the elaboration of silicon nitride based materials is achieved by sintering powders under a nitrogen atmosphere in order to limit the weight loss and the degradation of the silicon nitride based system. That is why a nitrogen atmosphere is used for heat treatment in the following sections. 3.1.2.2 Weight evolution under nitrogen atmosphere The aim of the use of nitrogen is to limit the weight loss by preserving the N content in the as-formed powders in order to further obtain dense silicon nitride based ceramic materials. Heat treatment was performed at 1000°C and then in steps of 100°C between 1300°C and 1700°C with a heating rate of 10°C/min. Most often, the dwell time is 4 h, unless otherwise indicated in the text. Previously, the as-formed Si/C/N powders (about 2 g) are slightly pressed in a Teflon mould to form pellets (diameter = 20 mm; height ≈ 10 mm) which are then placed in graphite crucibles located inside the graphite furnace. For Si/C/N nanopowders synthesised from the gas phase (SiCN29 and SiCN35), a significant mass change (+8 wt%) is obtained for the SiCN35 sample between 1200°C and 1400°C suggesting the nitridation of the free Si present in the powder. Contrary to the SiCN35 sample, the SiCN29 sample exhibits a relative mass stability up to 1600°C (Mayne 1997). This can be related to the high N content and to the absence of Si that cannot enable a nitridation process (Mayne 1997; Mayne et al. 1998). X-ray diffraction (XRD) patterns of the annealed powders show the presence of crystalline phases (α- and β-Si3N4 for SiCN29 sample and a mixture of α- and β-Si3N4 with β-SiC for SiCN35 sample). In contrast to Si/C/N nanopowders obtained from the gas phase, Si/C/N and Si/C/N/Al/Y/O powders obtained from the liquid phase (HMDS or mixtures of HMDS with organic compounds) exhibit weight losses that are of the same order of magnitude (20–30% at 1600°C). Therefore, the weight evolution of Si/C/N/Al/Y/O powders (Cauchetier et al. 1999; Mayne et al. 1999), will not be specifically presented in this chapter. Such weight losses suggest a decomposition of the Si/C/N chemical system even under nitrogen atmosphere. In Table 3.1.1, the weight losses and chemical compositions of six HMDS samples are given. It shows that the weight loss is dependent on the chemical composition of the as-formed powder. After annealing at 1600°C, the weight loss is the highest for the samples with the highest C/N ratio. This difference could be related to different chemical mechanisms involved in the decomposition process and interpretations will be suggested in the TG–MS section. This study on the weight evolution of Si-based samples during heat treatment enables us to show the following: • a strong difference in the behaviour of powders obtained from the gas phase or from the liquid phase using the aerosol method especially under a nitrogen atmosphere. Nanopowders obtained from the gas phase are more stable than those obtained from the liquid phase, which suggests that they are more suitable for ceramic conversion than those obtained from the liquid phase; • that the thermal behaviour of powders obtained from the liquid changes as a function of the chemical composition of the powder, suggesting different mechanisms.
< previous page
page_27
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_27.html [20/01/2010 10:03:17 AM]
page_28
< previous page
page_28
Page 28 Table 3.1.1 Results of chemical analyses for HMDS40 to HMDS45 Heating treatment (°C) Mass loss (%) HMDS40 AFa 1000 1300 1400 1500 1550 1600 HMDS41 AFa 1000 1300 1400 1500 1550 1600 HMDS42 AFa 1000 1300 1400 1500 1550 1600 1700 HMDS43 AFa 1000 1300 1400 1500 1550 1600 1700 HMDS44 AFa 1000 1300 1400 1500 1550 1600 1700 HMDS45 AFa 1000 1300 1400 1500 1550 1600
next page > Si
C
N
O
∑b
N/ C/ C/N Si Si
—46.725.021.8 5.948.423.620.9 5.751.323.723.7 6.051.523.722.5 19.459.626.812.6 27.065.728.2 4.7 27.968.629.1 2.9
6.1 99.60.931.24 1.33 5.0 97.90.861.14 1.31 2.2100.90.921.07 1.16 1.5 99.20.871.07 1.23 0.7 99.60.421.05 2.47 0.8 99.40.141.00 7.02 0.5101.10.081.0011.15
—46.120.625.2 4.450.419.323.5 5.851.419.227.3 7.452.518.727.0 17.259.221.019.6 28.661.623.111.8 28.267.425.2 8.5
6.7 98.61.091.04 4.6 97.80.930.89 2.4100.31.060.87 1.7 99.91.030.83 1.1100.90.660.83 1.1 97.60.380.87 1.4102.40.250.87
0.95 0.95 0.82 0.81 1.25 2.28 3.50
—44.418.729.7 4.048.917.927.1 5.951.618.329.5 8.052.618.029.8 14.655.818.422.1 23.465.220.913.1 27.067.222.511.5 28.866.623.3 9.7
7.7100.51.340.98 4.4 98.31.110.85 1.5100.91.140.83 1.6102.01.130.80 0.8 97.10.790.77 1.0100.20.400.75 1.0102.20.340.78 0.3 99.90.290.81
0.73 0.77 0.72 0.70 0.97 1.85 2.27 2.80
—48.315.526.8 4.750.213.830.3 8.053.214.031.5 10.854.314.428.2 18.058.313.026.9 25.358.813.227.3 25.265.416.719.3 28.864.219.417.1
8.0 98.61.110.75 5.9100.21.210.64 3.8102.51.180.61 2.9 99.81.040.62 1.4 99.60.920.52 0.7100.00.930.52 1.0102.40.590.60 0.4101.00.530.71
0.67 0.53 0.52 0.60 0.56 0.56 1.01 1.33
—47.113.026.710.9 97.71.130.64 6.249.811.132.5 7.4100.81.300.52 9.753.311.132.4 4.5101.31.210.48 12.752.610.532.4 3.4 98.91.230.46 19.159.0 9.829.7 2.0100.51.010.39 27.756.910.431.2 0.5 99.01.100.42 24.462.412.123.3 1.1 99.00.750.45 25.762.613.725.6 0.5102.40.820.51
0.57 0.40 0.40 0.38 0.38 0.39 0.61 0.62
—47.6 7.451.8 11.655.4 14.152.9 17.058.5 23.454.7 20.460.3
0.33 0.21 0.20 0.15 0.12 0.05 0.14
8.328.913.4 98.21.210.41 6.134.2 9.7101.81.320.27 5.732.4 5.9 99.41.170.24 4.735.8 4.9 98.31.350.21 3.635.9 0.9 99.01.230.14 1.634.4 0.6 92.31.260.07 4.233.8 1.3 99.61.120.16
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_28.html (1 of 2) [20/01/2010 10:03:18 AM]
page_28
Notes a As-formed powder. b The sum of the different element masses from 100% due to the uncertainty of the chemical analyses and the hydrogen is not taken into account, namely for the as-formed powders.
< previous page
page_28
next page >
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_28.html (2 of 2) [20/01/2010 10:03:18 AM]
page_29
< previous page
page_29
next page >
Page 29 The as-formed powders obtained from the gas phase are at least partially organised, and the weight changes occurring during thermal treatments are much less noticeable than for the powders obtained by the aerosol method from the liquid phase that are amorphous. 3.1.3 Chemical evolution during annealing in a nitrogen atmosphere As in the previous chapter, the chemical composition in stoichiometric compounds of the different samples annealed under a N2 atmosphere has been calculated from chemical analysis obtained from CNRS analysis laboratory (Vernaison, France). The knowledge of the composition in stoichiometric compounds (Si3N4, SiC, SiO2, Y2O3, Al2O3), especially for annealed powders is important, because it enables us to evaluate roughly the composition of future sintered materials. Moreover, this allows a more precise choice of the adapted powders to obtain the desired material with specific properties. The determination of the chemical composition in stoichiometric compounds for the different samples is as follows: for Si/C/N/Al/Y samples, all Al and Y are assumed to be in the form of Al2O3 and Y2O3, the remaining O being in the form of SiO2, then all N forms Si3N4 and the remaining Si is in the form of SiC. Free C is the difference between total C and C bonded to Si in SiC. The rules are the same for Si/C/N samples apart from Al and Y that are not present. It must be noted that such a calculation is approximate both for asformed and annealed powders. Effectively, in the case of amorphous as-formed powders, compounds such as Si3N4, SiC, Y2O3, Al2O3 do not really exist as crystalline compounds. In annealed Si/C/N powders, crystalline compounds Si3N4 and SiC exist but the crystallisation is not always complete, depending on the annealing temperature (as shown by XRD measurements). In Si/C/N/Al/Y/O powders, Al and Y are not only bonded to O (Y2O3, Al2O3) but may also be combined in SiAlON or YSiAlON amorphous phases (see Chapter 5), as for classical sintering of silicon nitride compounds in the presence of sintering aids (Y2O3, Al2O3) (Ekström and Persson 1990; Hoffmann and Petzow 1993). Note that the calculated Si3N4 and SiC contents should be very similar to that which exists in materials because of the low quantity of Y and Al bonded to N. Furthermore, H present in as-formed powders has not been taken into account for these chemical measurements. The chemical composition in stoichiometric compounds is presented for Si/C/N and Si/C/N/Al/Y powders, both obtained from the liquid phase in Tables 3.1.2 and 3.1.3. Tables 3.1.2 and 3.1.3 also give the C/N ratios in the as-formed powders, because they are often used in the following sections to characterise a sample. 3.1.3.1 Si/C/N samples The samples studied in this section have an initial C/N ratio in the range 0.2–2.6 (HMDS40–45 and HMDS36, 66 and 67). The chemical composition in atomic ratio (C/Si, N/Si and C/N) and its evolution as a function of annealing treatment between 1000°C and 1600°C is presented in Table 3.1.1 for samples HMDS40–45. The results for stoichiometric compounds after annealing at 1600°C, are reported in Table 3.1.2 for HMDS40–45 and HMDS36, 66 and 67. Part of these results appear in the PhD thesis of Emmanuel Musset (Musset 1995). Up to 1400°C, the chemical composition of Si/C/N samples presented in Table 3.1.1 shows no significant changes in the different atomic ratio values. Meanwhile, at higher temperatures
< previous page
page_29
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_29.html [20/01/2010 10:03:18 AM]
page_30
< previous page
page_30
next page >
Page 30 Table 3.1.2 Chemical composition (wt%) of various HMDS samples after annealing 1600°C assuming stoichiometric composition Samples Si3N4 SiC SiO2 C C/N (at) initial ratio HMDS36a 5.3 91.5 1.9 1.3 2.8 HMDS40 7.7 87.6 2.1 2.6 1.3 HMDS41 19.1 75.1 3.3 2.6 0.9 HMDS42 28.6 67.4 3.0 1.0 0.7 HMDS43 56.4 37.7 3.0 2.9 0.7 HMDS44 65.9 29.9 2.8 1.4 0.6 HMDS45 88.9 8.4 2.5 0.3 0.3 HMDS66 6.2 83.0 1.5 9.9 1.8 HMDS67 6.3 82.4 1.5 9.8 2.4 Note a Without ammonia in the carrier gas during synthesis. Table 3.1.3 Chemical composition of Si/C/N/Al/Y/O pre-mixed powders after annealing under N (1 h, 1600°C) assuming stoichiometric composition Powder sample Chemical composition (wt%) (Al + Y)/Si Al/Y C/N initial ratio Y2O3 Al2O3 SiO2 Si3N4 SiC C HSAl03 2.8 0 17.8 70.2 10.4 3.1 HSAl04 7.1 0 18.3 66.7 8.1 3.7 HSAl07 3.1 0 17.6 72.2 5.9 0.04 2.7 HSAl09 3.3 1.7 92.3 0.2 2.5 0.03 0.2 HSAl12 2.6 0.4 52.7 44.0 0.2 0.02 0.6 HSAl13 3.3 0.8 17.0 78.5 0.4 0.03 1.4 HSAl14 3.5 0.5 46.5 48.1 1.4 0.03 0.8 HSAl15 3.9 0 77.5 16.1 2.4 0.04 0.5 HSAlY05 1.3 3.8 0 19.3 64.1 9.0 3.5 HSAlY16 0.1 0.3 1.9 92.4 3.1 2.1 0.01 14.8 0.3 HSAlY17 0.6 0.9 1.4 51.9 43.7 1.5 0.01 3.2 0.8 HSAlY18 1.1 1.1 1.5 14.5 80.9 0.8 0.01 2.3 1.1 different evolutions occur depending on the initial C/N ratio (Tables 3.1.1 and 3.1.2): • For the C-rich samples (HMDS36, 66, 67 and HMDS40), the C/N atomic ratios compared to the as-formed powders increase and the powders are converted essentially towards SiC (between 80% and 90%) during annealing (C/Si atomic ratio near 1, see Table 3.1.1). Free C is always present in these samples after annealing at 1600°C (Table 3.1.2). • For the N-rich samples (HMDS44 and 45), the C/N atomic ratios decrease with a stabilisation of the N content and the powders are converted essentially towards Si3N4 (between 66% and 89%). • For the two samples with intermediate composition (HMDS42 and 43, initial ratio C/N = 0.7), the C/N atomic ratios remain relatively stable with a stabilisation or a slight decrease of the C/Si atomic ratios and a conversion of the powder towards a composite powder containing both SiC and Si3N4.
< previous page
page_30
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_30.html [20/01/2010 10:03:19 AM]
page_31
< previous page
page_31
next page >
Page 31 Whatever the composition of the initial powders, annealing induces a decrease in silica and in free C content because of the carbonitridation of this compound which involves CO evolution. For C-rich powders, the change in composition (Table 3.1.2) to SiC-rich compounds, during annealing at 1600°C under a N2 atmosphere, can be essentially linked to the decomposition of nitrogenous species (Si/C/ N, Si3N4) occurring from 1450°C. Such decomposition is important because of the high C content in asformed powders (C/N > 0.75) (Musset 1995; Musset et al. 1997). Effectively, extended X-ray absorption fine structure (EXAFS) (Chapter 5.4) and nuclear magnetic resonance (NMR) (Chapter 5.1) analysis of C-rich powders synthesised from HMDS have shown that the atomic local arrangement of Si is essentially composed of mixed SiC3N tetrahedra and of SiC4 tetrahedra which are already close to the SiC structure. This suggests the decomposition of slightly nitrogenous compounds (SiC3N) during annealing in order to reach the SiC structure. Moreover, annealing induces a decrease in silica and in free C content because of the carbonitridation of this compound which involves CO evolution. For N-rich powders, EXAFS and NMR analysis have shown that the atomic local arrangement is essentially composed of SiN4 tetrahedra which are the local environment of crystalline Si3N4. Therefore, the evolution towards a major phase of Si3N4 after annealing is not surprising. The drastic change between the evolution of Si/C/N towards SiC or Si3N4 compounds is observed for the initial C/N atomic ratio in the as-formed powders near the 0.75 value and corresponding to a 3SiC–Si3N4 mixture (Figure 3.1.1). 3.1.3.2 Si/C/N/Al/Y/O samples For samples obtained from a mixture of organometallic compounds as precursors, the comments are mainly focused on the aspects specific to the presence of Al and/or Y in the powders. Table 3.1.2 presents the results in stoichiometric compounds after annealing at 1600°C for 1 h under a N2 atmosphere for Si/C/N/Al/Y/ O samples with an initial C/N ratio in the same range as HMDS samples (0.2–2.6). The most important difference between Si/C/N samples obtained from only HMDS and Si/C/N/Al/Y samples obtained from a mixture of organometallic precursors is the incorporation of Al and Y metallic elements into the Si/C/N system, which could modify the evolution of the chemical composition of the Si/C/N system during annealing. That is why a comparison between Si/C/N and Si/C/N/Al/Y samples with a similar C/N ratio is presented below. Tables 2.6 and 3.1.3 clearly show that, in the Si/C/N/Al/(Y) systems, the Al+(Y)/Si ratios remain similar to those of the corresponding as-formed powders. This attests that the thermal treatment under a nitrogen atmosphere (1600°C) does not induce the degradation of all Al and Y containing species. Thus, Al and/or Y additives remain in the powder after annealing, which is important for the future sintering process, in which sintering aids (Y2O3, Al2O3) are necessary in order to obtain dense nanomaterials. By comparing, after heat treatment, HSAl or HSAlY samples (Table 3.1.3) with HMDS samples (Table 3.1.2), one can see that the evolution of the chemical composition in Si/C/N/Al(Y) system as a function of the C/N ratio is comparable to that in HMDS samples previously discussed. In this way, C-rich Si/C/N/Al/Y samples (initial C/N ratio between 1.1 and 2.7) are converted essentially to SiC (content between 64% and 81%, see samples HSAl03, 04, 07 and HSAlY05) while N-rich samples (C/N ratio between 0.2 and 0.3) are
< previous page
page_31
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_31.html [20/01/2010 10:03:19 AM]
page_32
< previous page
page_32
next page >
Page 32
Figure 3.1.1 Change in phase content (SiC, Si3N4, SiO2 and C) in HMDS powders after 4 h annealing under nitrogen at 1600°C. (Reprinted from Musset 1995.) converted essentially to Si3N4 (content of 92%, see samples HSAl12 and HSAlY17). Samples exhibiting an intermediate composition (C/N ratio between 0.6 and 0.8) are converted to a mixture containing both SiC and Si3N4 (SiC around 44 wt%, Si3N4 between 52% and 53%, see HSAl12 and HSAlY17 samples). Note that Crich samples also contain a noticeable quantity of free C (between 6% and 10%). Meanwhile, even if the evolution of the chemical composition is similar between Si/C/N and Si/C/N/Al(Y)O samples, noticeable differences appear where the C/N values and also the Si3N4 and SiC contents are concerned, especially for Si/ C/N and Si/C/N/Al/Y C-rich samples (C/N = 2.6). Figure 3.1.2 shows the evolution of the C/N ratio after a 1 h annealing treatment at 1600°C under a N2 atmosphere for some C-rich samples (HMDS66, HSAl03, 04 and HSAlY05). In this figure, the C/N ratio is around 15 for HMDS powders while it is only of 4.3–5.1 for HSAl(Y) powders. These results indicate that the loss of N is lower for powders containing Al and Y additives and exhibiting high C/N ratio. The SiC content is then lower and the Si3N4 content is higher in these Si/C/N/Al/(Y) O samples than those in Si/C/N samples (see Tables 3.1.2 and 3.1.3). This suggests that the decomposition of N containing species (Si/C/N, Si3N4) is limited during heat treatment of Si/C/N/Al/Y powders, probably due to the formation of a liquid phase in the
< previous page
page_32
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_32.html [20/01/2010 10:03:20 AM]
page_33
< previous page
page_33
next page >
Page 33
Figure 3.1.2 Evolution of the C/N atomic ratio with annealing temperature. (Reprinted from Cauchetier et al. 1999 with permission from Kluwer Academic/Plenum Publishers.) quaternary Si–Al–O–N or in the quinary Y–Si–Al–O–N diagram preventing the degradation of nitrogenous compounds. 3.1.4 Structural changes XRD and infrared (IR) measurements were carried out in order to obtain information about the nature of the different phases present and the evolution of structure and of the different chemical bonding after heat treatment. They were carried out on both Si/C/N and Si/C/N/Al/Y samples obtained from the liquid phase. 3.1.4.1 Si/C/N samples For annealing temperatures below 1500°C, the XRD diagrams of Si/C/N nanopowders (HMDS samples) are flat indicating that the powders are still amorphous. The IR spectra are very similar to the spectra of asformed powders (see for example Figure 2.8), apart from the absorption bands at 1170, 2950 and 1255 cm −1 involving hydrogenated bonds that disappeared. At 1500°C, peaks are present on the XRD diagram (Figure 3.1.3), indicating the presence of crystallised β-SiC in HMDS40, 41 and 42 samples and α- and β-Si3N4 phases in HMDS45. For HMDS43 and 44, the peaks are small and broad indicating a lower degree of crystallisation. Figure 3.1.4 presents IR spectra for three samples (C/N = 0.73, 0.67 and 0.57, respectively for HMDS42, 43 and 44) at the same temperature (1500° C). It shows two broad peaks centred near 900 and 500 cm−1 indicating the presence of an amorphous material and corresponding to Si—C—N and Si—N bonds, respectively. These results, together with the XRD result, indicate that crystallisation is not complete at this temperature, especially for samples with an ‘intermediate’ C/N ratio (HMDS43 and 44). This late crystallisation will be discussed in more detail in Chapter 5.5. Between 1500°C and 1600°C, noticeable changes occur both in the XRD diagram and in the IR spectra (Figures 3.1.4 and 3.1.5). Figure 3.1.5 presents the XRD diagrams of samples annealed at 1600°C. C-rich powders (HMDS41 sample) lead preferentially to the β-SiC phase, as was already noticed at 1500°C. N-rich powders (HMDS45 sample) mainly show
< previous page
page_33
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_33.html [20/01/2010 10:03:20 AM]
page_34
< previous page
page_34
next page >
Page 34
Figure 3.1.3 XRD patterns of HMDS powders after annealing at 1500°C. (Reprinted from Musset 1995.) the presence of α- and β-Si3N4 phases and very small β-SiC peaks. Samples exhibiting intermediate composition (HMDS43 and 44) lead to a mixture of SiC and Si3N4. In the IR spectra (Figure 3.1.4), the broad peak centred near 900 cm−1 becomes sharper between 1500°C and 1600°C. The shape becomes similar to the signature of crystallised SiC nanopowders obtained from the gas phase. The fine absorption bands present in the 800–400 cm−1 range indicate the crystallisation of N-rich powders only present in HMDS43 and 44 samples (α- and β-Si3N4 phases, Luongo 1983). These results (XRD and IR) are in good agreement with the calculated chemical compositions given in Table 3.1.2.
< previous page
page_34
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_34.html [20/01/2010 10:03:21 AM]
page_35
< previous page
page_35
next page >
Page 35
Figure 3.1.4 Change in IR spectra during annealing under nitrogen between 1500°C and 1700°C. (Reprinted from Musset 1995.) 3.1.4.2 Si/C/N/Al/Y/O samples As mentioned above for Si/C/N samples, annealing treatment under a nitrogen atmosphere also induces a drastic change in the structure of Si/C/N/Al/Y powders. From amorphous, in their as-formed state, they become crystallised or at least partially crystallised after a 1 h treatment at 1600°C under nitrogen atmosphere. Figure 3.1.6 shows XRD diagrams of Si/C/N samples (0.2 < C/N < 1.7) annealed under nitrogen at 1600°C for 1 h. The nature and the crystallographic variety of the phases that crystallise during heat treatment are very similar to those obtained from Si/C/N powders (HMDS samples). Thus, for a C-rich Si/C/N/ Al powder (HSAl13), the XRD diagram shows an evolution towards α- and β-SiC compounds while for a N-rich Si/C/N/Al powder (HSAl09), α- and β-Si3N4 are formed with a higher quantity of the α phase compared to the β phase. For samples having intermediate composition (HSAl12), α-and β-Si3N4 and β-SiC phases are formed. The IR spectra of the same samples (Figure 3.1.7) are in good agreement with the XRD diagram, that is to say that SiC bonds (around 900 cm−1) are detectable in a C-rich system, while Si N bonds in a Si3N4 structure are detectable in a N-rich system. The sample with intermediate composition contains the Si— N bonds in the Si3N4 structure and also Si—C bonds. IR and XRD results are very consistent with the chemical composition mentioned above. For C-rich samples (C/N = 2.6, HSAlY05 and HMDS66 samples), a comparison between the XRD diagrams of Si/C/N and Si/C/N/Al/Y powders annealed at 1600°C is presented (Figure 3.1.8). Moreover, the evolution of the IR spectra as a function of the temperature is presented for the same samples (Figure 3.1.9). XRD patterns of HSAlY05 and HMDS66 annealed at 1600°C are shown in Figure 3.1.8. The Si/C/N/Al/Y powder annealed for 1 h (HSAlY05 sample) presents broad diffraction
< previous page
page_35
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_35.html [20/01/2010 10:03:22 AM]
page_36
< previous page
page_36
next page >
Page 36
Figure 3.1.5 XRD patterns of HMDS powders after annealing at 1600°C. (Reprinted from Musset 1995.) lines of β-SiC that are indicative of a low degree of crystallisation (Figure 3.1.8(a)). There is also evidence for the presence of the α-SiC phase (2H polytype). When annealing time is increased, well-crystallised α-SiC (2H polytype) and β-SiC are present (Figure 3.1.8(b)). In contrast, for the Si/C/N powder (HMDS66 sample) there is evidence of α- and β-SiC even after only 1 h of annealing and no difference can be noticed in the diffractogram for an annealing duration of 1 or 4 h (Figure 3.1.8(c) and (d)). These results suggest that for Crich powders, the presence of Al and Y either limits the crystallisation or enables the formation of an amorphous phase initiated in the Y–Si–Al–O–N quinary system.
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_36.html (1 of 2) [20/01/2010 10:03:23 AM]
page_36
< previous page
page_36
next page >
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_36.html (2 of 2) [20/01/2010 10:03:23 AM]
page_37
< previous page
page_37
next page >
Page 37
Figure 3.1.6 XRD analysis of annealed HSAl powder. (Reprinted from Mayne et al. 1999.)
Figure 3.1.7 IR spectra of annealed HSAl powder. (Reprinted from Mayne et al. 1999.) Figure 3.1.9 presents examples of IR spectra of the as-formed and annealed Si/C/N and Si/C/N/Al/Y/O powders (high C/N ratio). Up to 1400°C, the spectra of Si/C/N/Al/Y/O powder are very similar to the spectra obtained for Si/C/N powder. The only difference seems to be a flat base line for the powders containing Al (+Y) additives whereas a pronounced dip appears near 1000 cm−1 in the IR spectrum of powders without additives
< previous page
page_37
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_37.html [20/01/2010 10:03:23 AM]
page_38
< previous page
page_38
next page >
Page 38
Figure 3.1.8 XRD patterns of samples (a) and (b) HSAlY05 and (c) and (d) HMDS66 after 1 and 4 h annealing under N at 1600°C. (Reprinted from Cauchetier et al. 1999 with permission Kluwer Academic/Plenum Publishers.)
Figure 3.1.9 Changes in IR spectra with annealing temperature. (Reprinted from Cauchetier et al. 1999 with permission Kluwer Academic/Plenum Publishers.) indicating crystallisation or grain growth as observed previously in the annealing of SiC powders obtained by a laser gas-phase driven reaction (Tougne et al. 1993) or from pyrolysis of a polycarbosilane (Sasaki et al. 1989). No significant change is observed when the dwell time increases from 1 to 4 h and no signature characteristic of Al or Y is observed. This study of chemical and structural changes during annealing of Si/C/N and Si/C/N/Al/Y/O samples under nitrogen atmosphere has shown a comparable evolution of Si/C/N and Si/C/N/Al/Y/O samples with comparable C/N ratio. A more detailed comparison seems to indicate that the presence of elements of sintering aids limits the degradation of the nitride phase during heat treatment of Si/C/N/Al/Y/O samples. Another point is that the elements Al, Y and O aids remain present in the powder after thermal treatment, which is encouraging for future elaboration of materials.
< previous page
page_38
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_38.html [20/01/2010 10:03:24 AM]
page_39
< previous page
page_39
next page >
Page 39 3.1.5 Information about changes in the grain sizes BET measurements were carried out in order to measure the specific surface area, which enables determination of the changes in reactivity and grain size after heat treatment. These measurements should be related to transmission electron microscopy (TEM) analysis (see Chapter 4). 3.1.5.1 Si/C/N samples Figure 3.1.10 shows the variation of only two Si/C/N samples (HMDS41 and HMDS44). Below 1000°C, the SBET decrease can be explained by the smoothing of the particles due to the reticulation reactions, which occur during the ceramisation of the powders. Then the SBET value remains constant up to 1400–1500°C and the decrease at 1600°C is due to the crystallisation and growth of the particles, as confirmed by TEM (Chapter 4). 3.1.5.2 Si/C/N/Al/Y/O samples Annealing (nitrogen atmosphere, 1600°C, 1 h) of Si/C/N/Al/Y/O powders induces a decrease of the specific surface area compared with that of initial powders attesting to a structural and morphological change during heat treatment such as crystallisation, structural modification of free C and particle growth. The difference between the specific surface areas of as-formed and annealed powders increase when the C/N atomic ratio decreases. Thus for C-rich Si/C/N/Al/O powders (HSAl07 sample), the specific surface area varies from 110 m2/g (as-formed) to 54 m2/g (annealed) while for N-rich Si/C/N/Al/O powders (HSAl09 sample), the decrease of the specific surface area is more important (112–12 m2/g). A similar evolution is also true for the series of Si/C/N/Al/Y/O samples. This phenomenon could suggest a different grain growth process in C-rich powders compared to N-rich powders, that is to say that the grain growth could be more pronounced in Nrich samples. Apart from a low grain growth,
Figure 3.1.10 Change in specific surface area during annealing under Nfora C-rich HMDS powder (HMDS41 sample) and a N-rich HMDS powder (HMDS44 sample). (Reprinted from Musset 1995.)
< previous page
page_39
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_39.html [20/01/2010 10:03:24 AM]
page_40
< previous page
page_40
next page >
Page 40 this could also be related to the low crystallisation degree (see XRD patterns above) and to a structural modification of free C giving rise to some C ribbons as was already observed (Musset 1995) and as is usually formed from the heat treatment of amorphous C between 1500°C and 2000°C (Dresselhauss et al. 1988). These interpretations must be checked by TEM observations in order to determine the main phenomenon responsible for the surface area results. 3.1.6 Conclusion From the first section of this chapter devoted to thermal behaviour, several interesting points can be noted: • The thermal behaviour of Si/C/N powders can be related to synthesis conditions; powders obtained from the gas phase appear more stable than powders obtained from the liquid phase using the aerosol method. • Heat treatment under nitrogen allows one to obtain crystallised powders with a chemical composition varying from a major phase SiC to a major phase Si3N4 with intermediate mixtures of SiC + Si3N4. • The Al, Y and O elements of sintering aids remain present in the Si/C/N/Al/Y/O powders after thermal treatment under N atmosphere. The behaviour of these powders is qualitatively comparable to the behaviour of Si/C/N powders with comparable C/N ratio. The presence of these in situ sintering aids can be very helpful to obtain homogeneous dense materials – their influence is presented in Chapter 7. References Cauchetier, M., Croix, O., Herlin, N. and Luce, M. (1994) Journal of the American Ceramic Society, 77, 993. Cauchetier, M., Armand, X., Herlin, N., Mayne, M., Fusil, S. and Lefevre, E. (1999) Journal of Materials Science, 34,1. Croix, O., Gounot, M., Bergez, P., Luce, M. and Cauchetier, M. (1991) Ceramics Today: Tomorrow’s Ceramics, Elsevier Science Publishers, Amsterdam, p. 1447. Dresselhaus, M. S., Dresselhaus, G., Sugihara, K., Spain, I. L., Golbert, H. A., Cardona, M. (1988) Graphite Fibers and Filaments, Springer Verlag. Ekström, T. and Persson, J. (1990) Journal of the American Ceramic Society, 73, 2834. Hoffmann, M. J. and Petzow, G. (1993) Materials Research Symposium Proceedings, 287, 3–14 Luongo, J. P. (1983) Journal of the Electrochemical Society, 130, 1560. Mayne, Martine (May 1997) Ph.D. Thesis, Limoges University, 97LIMO0021; http://thesenet.abes.fr Mayne, M., Balhoul-Hourlier, D., Doucey, B., Goursat, P., Cauchetier, M. and Herlin, N. (1998) J. Eur. Ceram. Soc., 18, 1187. Mayne, M., Armand, X., Cauchetier, M., Doucey, B., Bahloul-Hourlier, D. and Goursat, P. (1999) Ceramics: Getting in the 2000’s, Part B (Ed. P. Vincezini) Techna, Faenza, pp. 211–218 Musset, Emmanuel (Nov. 1995) Ph.D. Thesis, Paris-Sud Orsay University, 95PA112537; http://thesenet.abes. fr Musset, E., Herlin, N., Cauchetier, M. and Luce, M. (1997) Silicates Industriels, 62, 111. Sasaki, Y., Nishima, Y., Sato, M. and Okamura, K. (1989) Physical Review B: Condensed Materials, 40, 1762. Tougne, P., Hommel, H., Legrand, A. P., Herlin, N., Luce, M. and Cauchetier, M. (1993) Diamond and Related Materials, 2, 486.
< previous page
page_40
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_40.html [20/01/2010 10:03:25 AM]
page_41
< previous page
page_41
next page >
Page 41 3.2 Thermal reactivity of silicon-based nanopowders Djamila Bahloul-Hourlier, Benoît Doucey, Jean-Louis Besson and Paul Goursat 3.2.1 Introduction Si/C/N nanopowders may be converted into Si3N4/SiC bulk materials by consolidation and hot pressing. Several studies have been devoted to the synthesis of Si/C/N nanopowders and their sintering. However, only a few studies on the thermal decomposition of these preceramic nanopowders have been reported (Giorgi et al. 1996; Suzuki et al. 1995; Borsella et al. 1997; Mayne et al. 1998; Pan et al. 1999), in contrast to the situation with organometallic polymer precursors of Si/C/N ceramics (Burns et al. 1987; Blum et al. 1989; Han et al. 1992; Corriu et al. 1992; Schmidt et al. 1992; Lavedrine et al. 1991; Bahloul et al. 1993, 1997). It is well known that ultrafine powders can undergo structural changes when they are heated at specific temperatures. This is due to their high surface energy and non-equilibrium phases. A good knowledge of adsorbed species on the surface, the nature of chemical groups present in nanopowders and their reactivity during annealing may be used to further improve the colloidal processing, shaping and forming techniques and also to optimise sintering conditions and thus mechanical properties. The aim of the present work is to further clarify the effects synthesis conditions and chemical composition of the preceramic Si/C/N nanopowders have on their thermal stability while under different atmospheres. The synthesis conditions and chemical composition of the studied powders as well as their corresponding designation are reported in Table 3.2.1. The studied samples have a C/N ratio varying from 0.2 to 2.6. Various experimental techniques: thermogravimetric analysis coupled with mass spectrometry (TGA/MS), elemental analysis and X-ray diffraction (XRD) were used to follow the evolution of annealing in preceramic nanopowders. Table 3.2.1 Nanopowders chemical composition Powder % NH3 (cm3/min) Chemical analysis (wt%) Atomic ratio C/N Chemical composition (at %) Si C N O Al Al2O3 SiO2 Si3N4 SiC Si C N SiCN29 40 58 6 35 1 — 0.2 —1 87 8 — 4 — SiCN35 0 67 13 18 2 — 0.8 —4 45 45 6 — — HMDS35 40 51 6 38 5 — 0.2 —9 77 — — 6 8 HMDS66 0 51 32 15 2 — 2.4 —5 37 39 — 19 — HMDS73 10 52 13 25 10 — 0.6 —19 63 7 — 11 — HSAl07 0 47 29 13 9 2 2.6 412 32 33 — 19 — HSAl09 40 49 7 36 4 2 0.2 49 76 — — 7 6
< previous page
page_41
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_41.html [20/01/2010 10:03:25 AM]
page_42
< previous page
page_42
next page >
Page 42 3.2.2 Results and discussions 3.2.2.1 TG/MS analysis Figure 3.2.1 shows a comparison of the measured weight losses during the decomposition of the as-received Si/C/N preceramic nanopowders in flowing helium (He). At first sight, the results indicate a direct dependence of the ceramic yields on the synthesis conditions. Obviously, the overall weight loss is greater for the family of nanopowders produced from liquid precursor (HMDS) than for that obtained from gas reactant SiH4 (gas). The major weight loss variations basically evolve at high temperature (T > 1300°C), where extensive degradation of the preceramic nanopowders occurs (Figure 3.2.1). A combined TGA/MS study was then used to determine the identity of the evolved species at each step. On account of the large number of powders produced by particular synthesis conditions, it is not possible to illustrate here all the mass spectra. Only the data corresponding to the sample that exhibited the highest weight loss (HMDS35) will be given in detail. However, when differences exist, they will be compared with the other samples. The TG/MS analysis of HMDS35 under He is given in Figure 3.2.2. On heating from room temperature to 300°C, the weight loss of 1% corresponds to the simultaneous escape of water (M/z = 18, 17) and ammonia (M/z = 17, 16, 14). The intensity of water progressively diminishes with increasing temperature up to approximately 300°C, while ammonia seems to stabilise between 400°C and 600°C and then diminishes with further heating. The appearance of two shoulders at M/z = 17 is evidence for the occurrence of at least two different reactions.
Figure 3.2.1 TG profiles of different nanopowders pyrolysed under He flow.
< previous page
page_42
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_42.html [20/01/2010 10:03:26 AM]
page_43
< previous page
page_43
next page >
Page 43
Figure 3.2.2 TG–MS analyses of HMDS35 nanopowder pyrolysed under He flow. The escape of H2O and NH3 at low temperatures (less than 300°C) may be a consequence of the higher latent reactivity induced by the presence of the condensable ≡Si—NH2 and Si OH groups on the preceramic nanopowders (Equations 3.2.1, 3.2.2a, b). (3.2.1) (3.2.2a)
(3.2.2b) While the nitrogen (N) bridging may take place at low temperatures, the reaction between silanol surface groups to form oxygen bridges is known to take place above 350°C (Equation 3.2.3). (3.2.3) Nakamatsu et al. (1998) proposed the following reaction (Equation 3.2.4) to explain the simultaneous desorption of both H2O and NH3 at low temperatures (around 200°C). (3.2.4) Besides NH3 and H2O, some other fragment ions at M/z = 44, 30 are also detected below 400°C. The intensities of these peaks are very low and thus prevent a detailed characterisation of the origin structures. Between 300°C and 900°C, a second weight loss (3.8%) is attributed to the second escape of ammonia (M/z = 17, 16), which indicates the occurrence of the
< previous page
page_43
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_43.html [20/01/2010 10:03:27 AM]
page_44
< previous page
page_44
next page >
Page 44 transamination/condensation reactions (Equation 3.2.5) which are known to occur during the thermal conversion of polysilazanes (Bahloul 1993).
(3.2.5) Concomitant with the evolution of NH3 is the loss of other gases with M/z varying from 42 to 12 atomic mass units (AMU) (Figure 3.2.3). It is noteworthy that compounds with molecular weights higher than M/z = 42 were not detected. Looking at these peak fragments, one would attempt to assign them to light hydrocarbons containing up to three carbon (C) atoms at most, like alcyne, olefin and alkane compounds. However, it should be remembered that the synthesis of this powder was made with NH3 as a reactant gas, being very reactive over Si—H, Si—C and C—C bonds. Consequently, the probability of formation of hydrocarboned species having two or three carbons in their structure seems very weak (Van Dijen and Pluijmakers 1989). Moreover, it is seen from the comparison of the intensities of the obtained peaks that the most intense peak at M/z = 41 is followed, by descending order in intensity, by the peak at M/z = 40, then M/ z = 39, and finally M/z = 42. No hydrocarbon combination with two or three carbons leads to such an evolution. It is, therefore, believed that these fragments may be assigned to R—C≡N species such as CH3 CN (M/z = 41, 40, 39, 38), HCN (M/z = 26, 27) and also to less protonated species such as carbo-imines like CH3 —CH=NH (M/z = 42, 28). Further data that confirms the assignment of such species will be presented during the analysis of the exhaust gas at high temperatures (T > 900°C).
Figure 3.2.3 MS analysis of HMDS40 nanopowder pyrolysed under He flow.
< previous page
page_44
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_44.html [20/01/2010 10:03:27 AM]
page_45
< previous page
page_45
next page >
Page 45 The maximum desorption of these species is situated at 600°C, whereas in the temperature range (600–900° C) the major volatile products detected are methane (M/z = 16, 15, 14) and H2 (M/z = 2). Methane continues to evolve up to 1000°C, whereas hydrogen evolution occurs in a wider temperature range up to 1500°C with a maximum loss at about 900°C. Some of these gaseous emissions are classical during the thermal conversion of polycarbosilane and polycarbosilazane polymers and were described by several authors whereas others are more specific to this type of laser-driven powders. Considering this temperature range, the reactions that describe the thermal decomposition of these materials are those that most probably involve radical mechanisms. There are several potential sources of radical species that can explain the above exhausted molecules (Equation 3.2.6–3.2.12). (3.2.6) (3.2.7) (3.2.8) (3.2.9) (3.2.10) (3.2.11) (3.2.12) For example, the formation of CH3—C≡N arises from radical cleavage of Si—CH2—C≡N leading to the •CH2— C≡N radical, followed by H abstraction and/or radical combination reactions. The formation of the other species can also be explained using this approach. The C—N≡groups do not appear in the initial structure of HMDS precursors, and seem to have been formed during the synthesis process. This is confirmed by Rice’s studies (1986) on the laser induced dissociation of the molecule of HMDS in the gas phase under argon. Analysis of gases of the processing chamber indicated the presence of, amongst other species, HCN and hydrocarbons, in particular. Thus, it is not surprising to think that, in our case, as the synthesis is being carried out in the presence of NH3, the concentration of C—N≡or amine groups giving HCN and RCN species, should increase at the expense of C—C groups yielding to light hydrocarbon species. Indeed, the reaction of C or hydrocarbon compounds with ammonia has been well described elsewhere and the resulting product is HCN while no hydrocarbons are formed (Corriu et al. 1992; Bahloul et al. 1993). Above 900°C, a significant weight loss is observed. This is accompanied by the increased evolution of the shape of the TGA curve. Between 900°C and 1400°C, besides H2, the major gaseous decomposition product is unambiguously ascribed to HCN at M/z = 26, 27. This exhaust gas gives credence to the description given above concerning the attribution to HCN and amine species of the signals at M/z between 42 and 12 AMU. This result is in good agreement with the chemical analysis of the as-received HMDS35 (Table 3.2.1) from which an excess of N and C are obtained assuming that only the equilibrium phases SiO2, SiC, Si3N4 and C, are present in the as-prepared powders (rule of mixture calculations). Furthermore, the short-range atomic structure description of the same Si—C—N nanopowders by XAS reveals the presence of C—N bonds in the amorphous network (Ténégal et al. 1996). A structural model has been proposed (Ténégal et al. 1996), where mixed tetrahedral SiCxN4−x are randomly linked through C—N bonds. The release of HCN at high temperature is further
< previous page
page_45
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_45.html [20/01/2010 10:03:28 AM]
page_46
< previous page
page_46
next page >
Page 46 proof that CN groups are not only pendant groups X—CN as observed for temperature T < 900°C, or radical scavenger/quencher groups under the experimental conditions employed in the synthesis process, but the branching groups to probably a mixed tetrahedra SiCxNy. Homolytic cleavages of C—N bonds between two mixed tetrahedra of silicon need more energy in comparison with those at chain-ends. Parallel to the evolution of HCN gas is the loss of N2 at M/z = 28, 14 up to the temperature limits of the experiment (1500°C) whereas the CO loss at M/z = 28, 12 begins at 1450°Cin minor amounts (comparison of ions at M/z = 12 for CO and M/z = 14 for N2). At 1500°C, despite the important weight loss, the intensity of N2 diminishes rapidly, some traces of CO are still detected by MS during the isothermal holding. Interestingly, at 1500°C, during the holding time, we observe that the mass continues to decrease with increasing time, whereas any species cannot be detected by MSin large enough quantities to account for this continued weight loss. It is believed that this weight loss in the TGA curve is due to compounds such as SiO which condense rapidly in cold parts of the apparatus and may not be detected by MS. Evidence for this proposal comes from the deposition of SiO as a wool-like product on many parts of the apparatus, which consequently leads to the breaking of the thermocouple based on platinum. The most probable chemical reactions in the Si/C/N/O system, that involve the evolution of volatile species and which produce a significant weight loss, can be described in two steps. Primarily, decomposition of the quaternary SiCxNyOz phase leads to the formation of an intermediate ternary oxynitride solid phase SixNyOz and the simultaneous release of SiO and CO, N2, in which N2 is the gas detected in the greatest quantity by MS. Then, in the second step, which occurs during holding at 1500°C, the oxynitride phase SixNyOz undergoes a decomposition in which gaseous N2, Si(l, g), SiO and a solid phase are produced according to the following reactions:
(3.2.13) The most known ternary oxynitride phase is Si2N2O. Although several investigators have reported on the thermal decomposition of Si2N2O, no mechanism has yet been clearly established. This is due to some of the following experimental difficulties: (a) the reproducibility of experiments, (b) the error in the determination of the weight loss, which is sometimes not representative of the real value of mass loss due to the condensation of the SiO species on the rod attaching the crucible to the balance, (c) progressive clogging of the aperture of the tube furnace and capillary for admission of gas to the mass spectrometer, by the deposit of SiO, and (d) the rupture of the thermocouple, stopping subsequent treatment. The majority of decomposition reactions of Si2N2O suppose the simultaneous escape of volatile species SiO(g) and N2(g). Our analyses revealed that, after 10 min at 1500°C, no gas species are detected by MS, despite the continued weight loss as observed by TGA. It may be assumed that as the powder HMDS35 has been synthesised with ammonia as a reactant, a noticeable number of SiN4 sites are present and the amount of C in this powder is low. Taking into account our previous observations, it is thus hypothesised that the oxynitride SiNxOy resulting from the decomposition of oxycarbonitride phase SiNxOyCz coexists with SiN4 sites initially present in the material. Hence when the duration of heating is increased, the oxynitride phase degrades to give SiO evolution in greater quantity, while the two other species
< previous page
page_46
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_46.html [20/01/2010 10:03:28 AM]
page_47
< previous page
page_47
next page >
Page 47
Figure 3.2.4 XRD patterns of nanopowders pyrolysed under a reactive (20%N2/He) and inert (He) atmosphere. Si(l, g) and N2 interact on the SiN4 sites to give better organised Si3N4 as supported by XRD illustrated in Figure 3.2.4. Rocabois et al. (1996) used Knudsen effusion MSto study the thermal degradation of several systems based on Si like binary, tertiary and even quaternary ones containing Si/C/N/O (Rocabois 1993). They stressed that the thermal degradation of Si-based materials is much less pronounced than what is predicted by thermodynamics and that their vaporisation is hindered and related to the different evaporation coefficients of each species. Moreover, the grain size, chemical composition, surface of contacts or interfaces during vaporisation would play an important role in the degradation of various phases. In our case, the nanopowder is initially amorphous as shown by XRD (Figure 3.2.4) and we can postulate that the number of surface contacts is high and the degradation of material is more homogeneous. By admitting, as suggested by Rocabois et al. (1996), that the evaporation coefficient of N2 is low in comparison with that of SiO, the two concomitant reactions, decomposition of oxynitride phase with release of SiO, Si(l, v), and N2, and the reaction of the two latter gaseous species on SiN4 sites initially present leading to new Si3N4 by epitaxial growth, is expected. 3.2.2.2 Major differences in thermal behaviour of the preceramic nanopowders The results pointed out major differences between the nanopowders synthesised from the same HMDS precursor with NH3 (HMDS35 and HMDS73) or without (HMDS66). Elemental
< previous page
page_47
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_47.html [20/01/2010 10:03:29 AM]
page_48
< previous page
page_48
next page >
Page 48
Figure 3.2.5 MS analysis of HMDS nanopowders pyrolysed under He flow. analysis of these powders confirmed that when NH3 is used during synthesis, the C/N ratio decreases. This diminution of C also depends on the concentration of NH3 in the reactant gas mixture. Moreover, during the heat treatment of these powders, the MS analysis also confirmed that the powders synthesised in the presence of NH3 contain more N—X bonds (X = H, C, Si). Indeed, the evolution of NH3 at M/z = 17 (Figure 3.2.5) occurs over a wide temperature range and is characterised by two waves for HMDS35 and HMDS73, whereas for HMDS66, it exhibits only one narrow wave up to 300°C. In the case of HMDS66 between 400°C and 700°C, the MS spectra (Figure 3.2.6) reveal the loss of Sicontaining species at M/z = 73, 59, 45, 44, 30, which suggests the formation of (CH3)x≤4Si, whereas for HMDS35 and HMDS73, species with M/z greater than 42 AMU were not detected. In view of the abundance of such organosilicon species, it seems that under the experimental conditions used during synthesis, the laser interaction with HMDS does not induce the total atomisation (bursting) of the molecular structure since NH3 is more reactive toward Si—C, which implies the amination of Si and C sites. This is the first, chief origin of the formation of N-rich powders. Above 800°C, it can be seen that for preceramic powders prepared in the presence of NH3 during the laser synthesis process, HCN evolves in larger quantities compared to the powders prepared without NH3.
< previous page
page_48
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_48.html [20/01/2010 10:03:30 AM]
page_49
< previous page
page_49
next page >
Page 49
Figure 3.2.6 MS analysis of HMDS nanopowders pyrolysed under a He flow. It can also be observed, that as the temperature increases (T > 1200°C) the release of N2 and CO illustrated in Figure 3.2.6 for the C-rich powder HMDS66 and the N-rich powder HMDS35 is different. Indeed, the release of N2 and CO takes place during the entire thermal cycle for HMDS66, whereas no gas is detected after 10 min at 1500°C for HMDS35 N-rich powder. This suggests that the thermal degradation of these two nanopowders proceeds according to different reaction paths and depends on the chemical composition as well as on the microstructure of the materials. The CO response for C-rich powder HMDS66 was not monomodal indicating that the process involves more than one reaction. The oxynitride intermediate phase suggested for a N-rich powder in reaction (3.2.13) would not be formed, since an excess of C is present. Regarding previously discussed thermal decomposition of silicon carbonitride material containing free-carbon phase obtained from polysilazane precursors, degradation of C-rich nanopowders may be related to the following reaction (Bahloul 1993):
(3.2.14) The loss of CO starts at about 1150°C, whereas the escape of N2 is observed from 1300°C. This can be explained in analogy to the reaction (Equation 3.2.15) observed in the solid phase
< previous page
page_49
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_49.html [20/01/2010 10:03:30 AM]
page_50
< previous page
page_50
next page >
Page 50 by the carboreduction of Si O bonds by excess C. (3.2.15) In an analogous fashion, the large amount of N2 evolved during the holding time at 1500°C can be explained by the reaction of Si—N and C: (3.2.16) Several authors (Rocabois et al. 1996; Lee and Jacobson 1992) have suggested that this reaction is inhibited when a SiC layer is formed on the surface of the C. This causes the system to shift to the equivalent SiC/ Si3N4 system and the excess loss of N2 would be suspected from the direct decomposition of Si3N4 as shown in the following equation: (3.2.17) It was supposed that, as the experimental procedure of heat treatment is the same for all powders, we should expect that N-enriched powders generate more N2 than C-enriched powders, since they contain more Si3N4 phase. This was not the case. Consequently, the decomposition of Si3N4 is not able to offer an explanation for the evolution of N observed. Furthermore, powder samples after heat treatment showed no evidence for the presence of metallic silicon when examined by XRD (Figure 3.2.4). SiC is one of the main compounds in the samples obtained from C-rich powder HMDS66 heated at 1500°C under He. The low emission of CO during holding time can be attributed to the following reactions: (3.2.18) (3.2.19) We, therefore, suggest that in our system the SiC obtained from the reaction of Si3N4 with C (3.2.16) may be consumed by SiO2 following reaction (3.2.18), which in turn releases C particles and consequently allows reaction (3.2.16) to continue producing gaseous N2. 3.2.2.3 Thermal behaviour of nanopowders under a nitrogen atmosphere The reason for studying the heat treatment under N was to answer the question: could the decomposition of silicon carbonitride, occurring under He, be stopped by using N environmental gas? The structural evolution of various nanopowders was thus followed as a function of heat treatment temperature and time whilst under a N atmosphere. The resulting curves in Figure 3.2.7, which represent the sole nanopowders that have the same ratio C/N = 0.2, show that below 1300°C the weight losses are nearly identical regardless of the nature of the atmosphere (nitrogen or He for the same kind of powder). The main gases detected by MS are attributed to the same species as those detected under He. In contrast, above 1400°C, comparison of the variation of mass is noticeably lower under N than He, as is shown for the HMDS35 sample. These differences are more pronounced for SiCN nanopowders obtained from only gaseous reactants (SiH4 + CH3NH2 + NH3 + Ar), as shown in the data in Table 3.2.2. The volatile species which evolve are similar to those obtained under He with a majority of CO but of a lesser degree. Furthermore, it can be seen from Figure 3.2.8 that the variation
< previous page
page_50
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_50.html [20/01/2010 10:03:31 AM]
page_51
< previous page
page_51
next page >
Page 51
Figure 3.2.7 MS analysis of HMDS nanopowders pyrolysed under He flow. Table 3.2.2 Nanopowders weight loss changes according to atmosphere heat treatment Atmosphere heat treatment Weight loss ΔM/Mo (%) SiCN35 SiCN29 HMDS66 HMDS35 HSAl07 HSAl09 He −7.7 −6.8 −16.3 −19.3 −20.6 −19.8 20%N2/He +6.1 +1.3 −6.2 −15.5 −14.6 −13.1 of mass is remarkably decreased with increasing partial pressure of N. These results suggest that carbothermal nitridation reactions take place at high temperatures under N according to the following reactions (Mayne et al. 1998): (3.2.20)
< previous page
page_51
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_51.html [20/01/2010 10:03:31 AM]
page_52
< previous page
page_52
next page >
Page 52
Figure 3.2.8 TG profiles of different nanopowders pyrolysed under a 20%N2/He flow. For C-enriched powders that contain more SiC phase, the nitriding process is also possible via the following reaction: (3.2.21) The weight gain observed, particularly for SiCN synthesised from gaseous reactants, can be attributed to the nitridation reaction of excess metallic silicon detected by XRD (Mayne et al. 1998). According to the α- or βSi3N4 content calculated from XRD patterns of heat treated powders, the nitridation reaction leads to the preferential formation of the α phase. This could be explained by an oversaturation in nitrogen coming from the nitrogen atmosphere, which results in the crystallisation of the less ordered α phase. Meanwhile, the β silicon nitride phase that is more ordered and stable, is preferentially formed during annealing under the inert He atmosphere. 3.2.2.4 Influence of the nature of the precursors’ source of silicon on the chemical composition and thermal stability It is observed that the aluminium doped powders (HSAl), synthesised under the same conditions as that of HMDS powders, except that only aluminium isopropoxide precursor is added, exhibit similar behaviour. Likewise, the differences observed between HMDS nanopowders and their conditions of synthesis, in particular the NH3 pressure in the reactive mixture of synthesis, seem to be reproduced for the HSAl powders. The role of aluminium isopropoxide introduced during the synthesis on the thermal behaviour is being studied. The use of a gas source of Si such as SiH4 has led to nanopowders of a more stable nature in terms of temperature, without doubt, due to their crystallisation state as revealed by XRD.
< previous page
page_52
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_52.html [20/01/2010 10:03:32 AM]
page_53
< previous page
page_53
next page >
Page 53 The formation of CN bonds does not seem to be favoured when SiH4 is used. However, contrary to the HMDS and HSAl powders, the use of silane (SiH4) generates an excess of metallic silicon within the powders, which will be used profitably during sintering under N. 3.2.3 Conclusion These studies indicate that the relative atomic concentrations of Si, C, N and H are primarily influenced by the types of carrier gases used for the synthesis laser process. Residual functionalities C—H, N—H and Si—H bonds will still be present as supported by the identification of volatile species by MS. The study of heat treatment of such systems based on Si indicates that thermal degradation is not an individual reaction but the net result of many reactions. The difference in thermal behaviour is attributed to variations in the preceramic structure. Taking into consideration the gases detected during our investigation and comparing them with similar results found by other research groups (9, 7), we are able to put forward the suggestion that by analysing preceramic nanopowders by thermal decomposition, it is possible to identify the processes by which they were synthesised. A potential advantage of laser-driven synthesis of refractory materials over gaseous reactants is the ability to include additives and co-reactants (e.g. sintering aids) (Cauchetier et al. 1999) in a truly homogeneous fashion. References Bahloul, D., Pereira, M. and Goursat P. (1993) J. Am. Ceram. Soc., 76(5), 1156–68. Bahloul, D., Pereira, M. and Gerardin, C. (1997) J. Mater. Chem., 7(1),109. Blum, Y. D., Schwartz, K. B. and Laine, R. M. (1989) J. Mater. Sci., 24, 1707. Borsella, E., Botti, S., Martelli, S., Alexandrescu, R., Cesile, M. C., Nesterenko, A., Giorgi, R., Turtu, S. and Zappa, G. (1997) Silic. Indus., 1–2,3. Burns, G. T., Angelotti, T. P., Hannemen, L. F., Chandra, G. and Moore, J. A. (1987) J. Mater. Sci., 27, 4651. Cauchetier, M., Armand, X., Herlin, N., Mayne, M., Fusil, S. and Lefevre, E. (1999) J. Mater. Sci., 34(21), 5257. Corriu, R. J. P., Leclercq, D., Mutin, P. H. and Vioux, A. (1992) Chem. Mater., 4, 711. Giorgi, R., Turtu, S., Zappa, G., Borsella, E., Botti, S., Cesile, M. C. and Martelli, S. (1996) Appl. Surf. Sci., 93, 101. Han, H. H., Lindquist, D. A., Haggerty, J. S. and Seyferth, D. (1992) Chem. Mater., 4, 705. Lavedrine, A., Bahloul, D., Goursat, P., Choong Kwet Yive, N. S., Corriu, R. J. P., Leclercq, D., Mutin, P. H. and Vioux, A. (1991) J. Eur. Ceram. Soc., 8, 221. Lee, K. N. and Jacobson, N. S. (1992) Ceram. Eng. Sci. Proc., 16th Ann. Conf. ou Comp. and Adv. Ceram. Mater., Cocoa-Beach. Mayne, M., Bahloul-Houlier, D., Doucey, B., Goursat, P., Cauchetier, M. and Herlin, N. (1998) J Eur Cer Soc, 18(9), 1187. Nakamatsu, T., Saito, N., Ishizaki, C. and Ishizaki, K. (1998) J. Eur. Ceram. Soc., 18, 1273. Pan, Z. W., Xie, S., Wang, G., Li, H. L. and Zhang, L. T. (1999) J. Mater. Sci., 34, 3047. Rocabois, P., Chatillon, C. and Bernard, C. (1996) J. Am. Ceram. Soc., 79(5), 1351. Rocabois, Philippe (1993) PhD, I.N.P.G., 93INPG; httl://thesenet.fr Rice, G. W. (1986) J. Am. Ceram. Soc., 69(8), C183. Schmidt, W. R., Marchetti, P. S., Interrante, L. V., Hurley, W. J., Lewis, R. H., Doremus R. H. and Maciel, G. E. (1992) Chem. Mater., 4, 937. Suzuki, M., Hasegawa, Y., Aizawa, M., Nakata, Y. and Okutani, T. (1995) J. Am. Ceram. Soc., 78(1), 83. Ténégal, F., Flank, A.-M. and Herlin, N. (1996) Phys. Rev. B, 54(17), 12029. Van Dijen, F. K. and Pluijmakers, J. (1989) J. Eur. Ceram. Soc., 5, 385.
< previous page
page_53
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_53.html [20/01/2010 10:03:32 AM]
page_54
< previous page
page_54
next page >
Page 54 4 Structure of some nanopowders and micro/nano composites by transmission electron microscopy Marc Monthioux, Catherine Béraud and Nahida El Horr 4.1 As-prepared and heat-treated nanopowders Some of both the raw and heat-treated powders were investigated by transmission electron microscopy (TEM). Sample preparation prior to TEM investigations and TEM operating conditions are reported in Section 4.3, together with a brief reminder of the principles for the various TEM modes used in the study. 4.1.1 Synthesis from gaseous precursors Starting from a mixture of silane (SiH4) and ethylene (C2H2) as gaseous precursors, a serie of SiC-based powders was obtained. Likewise, still using silane as Si source but replacing ethylene by ammonia (NH3) and/ or CH3NH2 allowed Si/C/N-based powders to be obtained. Si/C-based powders Materials were investigated either as-prepared or after various treatments. Related preparation conditions and elemental analysis of the as-prepared materials are reported in Tables 2.2 and 2.3, respectively. Some of the samples reported in Table 2.2 were investigated after various treatments, including SiC173, SiC177 and SiC212. Various annealing in argon atmosphere were carried out, in order to check structural and textural changes in both the SiC and C phase. Also, SiC173 and SiC212/1200 were investigated after thermal treatment at 450°C performed in air (1–3 h isothermal), in order to eliminate the carbon (C) phase when present. Finally, further heat-treatment experiments in inert atmosphere were also performed at 1800°C on sample SiC173 oxidised. Special precautions were taken for the 1800°C heat-treatment experiments (Laanani 1997) to prevent any possible oxidation reaction due to oxygen traces in the gas phase, that is, a non-dynamic, high purity argon atmosphere (N56 grade from Air Liquide) and an all-graphite furnace were used. SIC173, AS-FORMED Daylight colour of the as-prepared powder is dark grey, somewhat related to the polyaromatic C content, as already expected from the elemental analysis (see Section 3.1.1) and as supported in the following by the direct evidence from TEM investigation. Grains exhibit round and isometric shapes (Figure 4.1).
< previous page
page_54
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_54.html [20/01/2010 10:03:33 AM]
page_55
< previous page
page_55
next page >
Page 55
Figure 4.1 TEM bright-field image from SiC173. Arrows show stripes on SiC crystals indicating polytypes as stacking faults.
Figure 4.2 TEM lattice fringe image from SiC173. Note how two adjacent SiC crystals are able to accommodate a slight mismatch in orientation of their respective lattices, making both the 111 lattice fringes connected to each other without interruption. Grain sizes range according to a two-mode distribution. Large grains (10–60 nm) are prevalent, each being a single crystal, sometimes faulted (Figure 4.1, arrows). Grains are associated into aggregates, most often chain-like, due to both weak forces (electrostatic) or stronger ones, that is, structural. Figure 4.2 illustrates the latter, showing two grains whose lattices are connected despite a misorientation of 10°, obviously inducing a strong (covalent) bonding between grains. They are SiC crystals, β structure mainly, but some stacking faults
< previous page
page_55
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_55.html [20/01/2010 10:03:34 AM]
page_56
< previous page
page_56
next page >
Page 56 (indicating the local occurrence of polytypes) are revealed in electron diffraction patterns as additional aligned spots (Figure 4.3), as a probable consequence of the rapid growth. Grains are coated with a thin (~1 nm) layer of an amorphous phase, assumed to be a silicon oxide, as supported by X-photon energy dispersive spectroscopy (X-EDS) measurement, whose spectra show the presence of the element O, in addition to Si and C as expected (Figure 4.4). 4nm–1
Figure 4.3 Electron diffraction of SiC crystals from SiC173. The structure is mainly β-SiC (see Figure 4.7 for diffraction ring identification). However, arrows show some aligned spots indicating stacking fault sequences. The occurrence of an amorphous coating at the grain surface (thickness ~1 nm) is probable, though confusion with overfocusing Fresnel fringes is possible.
Figure 4.4 X-EDS spectrum of SiC crystals from SiC173. The presence of O attests the occurrence of an amorphous silica layer associated to the SiC grains.
< previous page
page_56
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_56.html [20/01/2010 10:03:34 AM]
page_57
< previous page
page_57
next page >
Page 57 The minor occurrence of a silica phase is consistent with the results from elemental analysis (Table 2.3). On the other hand, small grains are a very minor phase, whose sizes (3–10 nm) are difficult to estimate from regular bright-field images. Dark-field images help in more easily appreciating the occurrence and size distribution of it, as compared to the major phase (Figure 4.5(c), arrows). They are not Si3N4 but possibly SiC crystals too, since they appear in Figure 4.5(c) while not in Figures 4.5(a) or (b). However, other small, minor crystals are also found, despite that the amount of it is too small to appear in the diffraction pattern, from which high-resolution images reveal fringes whose spacing is too large to match the SiC lattice distances (not illustrated). Rarity and concentration of this minor phase are such that identification was not possible. A third phase is found associated with the major (SiC) phase, more or less coating the grain surface, and identified as polyaromatic C. Its low proportion is such as it does not appear in the electron diffraction patterns when exposure times are appropriately chosen to reveal the SiC phase (Figure 4.3). However, its structure is most probably turbostratic (i.e. not having the three-dimensional structure of graphite), as assumed from its morphology and nanotextural characteristics. Lattice fringe imaging mode illustrates the latter (Figure 4.2). The C phase appears as thin, somewhat buckling and polygonal, ribbon-like graphene stacks. Using the parameters N (number of graphenes per stack) and L2 (length of the continuous, though distorted, d002 lattice fringe) to characterise the nanotexture of the C phase, as proposed by Oberlin (1989), the latter exhibits a rather low N values (N ~ 2–5) with respect to
Figure 4.5 TEM dark-field image sequence from SiC173. (a) and (b) correspond to ‘polyaromatic Cspecific’ (DF1) dark-field imaging conditions for two selected orientations. The selected orientation direction is indicated by the ‘=’ sign, that is, only graphene stacks displayed parallel to the ‘=’ sign are imaged. Graphene stacks appear as small bright rims between SiC crystals. (c) corresponds to ‘SiC-specific’ (DF2) dark-field imaging conditions. Arrows show the occurrence of the minor phase (probably SiC) as small size grains among the larger SiC crystals.
< previous page
page_57
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_57.html [20/01/2010 10:03:35 AM]
page_58
< previous page
page_58
next page >
Page 58 a rather high L2 value (up to 20–30 nm). As far as the existence of free edges of graphenes is unlikely, since inducing improbable dangling bonds, and since the so-called ribbons never appear twisted as genuine ribbons might be, the graphene stacks are believed to be walls of three-dimensional, somewhat polyhedral, polyaromatic C shells. These shells are likely to form under mechanisms related to the thermal and/or catalytic decomposition of a carbide phase for instance (Badami 1965; Oberlin and Rouchy 1971; Audier et al. 1981). Similar textures, whose nanotexture parameters are fairly consistent with those measured here, were also found in oxygen-free SiC-based materials obtained from heat-treated polycarbosilane (Delverdier et al. 1991; Laanani 1997). Low magnification, specific (i.e. using an objective aperture selecting some diffracted polyaromatic 002 beams) dark-field images (Figures 4.5(a) and (b)) illustrate the proportion and location of the C phase relative to the SiC grains, as the latter appear as round-shaped, grey to pale white objects while the former appears as bright, elongated, tiny spots (arrows) in which graphenes are oriented parallel to the elongation direction. Though not systematic, graphene stacks are often found oriented parallel to the grain surface. SIC177, 1200°C ANNEALED The daylight colour of the starting powder is dark grey. The material is very similar to SiC173/as-prepared. Slight discrepancies concern the distribution of grain size (one-mode instead of two-mode), and the size range (slightly larger: 10–100 instead of 10–60 nm). Another difference lies in the probable absence of the non-identified, crystallised, minor phase of SiC173. Instead, another minor phase is found, mainly amorphous since specific darkfield images show that it does not contain any crystallised phases, neither Si3N4 nor SiC (not illustrated). Considering the high diffusion contrast of this phase in dark-field images when the beam tilt angle corresponds to the Bragg angle for the 002 reflection of polyaromatic C, it is believed that this amorphous phase is enriched in poorly organised, turbostratic C, as expected from the transformation of a formerly amorphous C phase due to the annealing temperature (1200°C is actually far above the minimal carbonisation temperature – ~500–600°C – i.e. the temperature sufficient to transform any kind of nongaseous C precursor into polyaromatic solids). This phase is distinct from the better organised, polyaromatic, turbostratic C phase associated with the SiC phase (Figure 4.6). Figure 4.6 exhibits a C shell still partially filled with a SiC crystal (arrow), which strongly supports that the porous C phase originates from a carbide decomposition process. SIC212, 1200°C ANNEALED The daylight colour of the starting powder is dark grey. The sample is mainly made of agglomerated SiC grains with round shapes (see Figure 4.1 for reference). Grain size range is 3–40 nm, that SiC-specific darkfield images show with a probable two-mode distribution similar to that of SiC177/as-formed (see Figure 4.5 (c) for reference). The structure is strictly β since only diffraction rings corresponding to 111, 200, 220 and 311 reflections of β-SiC appear (Figure 4.7). SiC crystals are coated with amorphous silicon oxide, ~1.5 nm thick (Figure 4.8). The coating may help the SiC crystals to link to each other (Figure 4.8). However, although confusion with an amorphous or poorly organised C coating was unlikely due to the annealing temperature, an oxidation experiment was performed to ascertain the oxide nature of the coating (see below). Unlike SiC173/as-formed or SiC177/1200°C, the relatively well-organised, turbostratic, polyaromatic C phase associated to the SiC phase (see Figures 4.2 or 4.6 for reference) is not
< previous page
page_58
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_58.html [20/01/2010 10:03:36 AM]
page_59
< previous page
page_59
next page >
Page 59
Figure 4.6 TEM lattice fringe image from SiC177/1200. Arrow shows a small SiC crystal filling incompletely a polyaromatic C shell, supporting the hypothesis that the polyaromatic C phase between SiC grains originates from the early decomposition of some primary SiC crystals.
Figure 4.7 Electron diffraction of SiC crystals from SiC212/1200. The structure is exclusively β-SiC. found. Instead, a poorly organised, turbostratic, polyaromatic C phase is found, concentrated into a minor phase consequently exhibiting a nanoporous texture (Figure 4.9), assumed to be similar to that found in sample SiC177/1200. SIC177, 1500°C ANNEALED The thermal treatment did not induce any change but the average SiC grain size, which has increased mainly due to a coalescence mechanism by impingement according to
< previous page
page_59
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_59.html [20/01/2010 10:03:37 AM]
page_60
< previous page
page_60
next page >
Page 60
Figure 4.8 TEM lattice fringe image of SiC crystals from SiC212/1200. The amorphous, about 2 nm wide silica coating is imaged, somewhat bonding crystals together.
Figure 4.9 TEM bright-field image from SiC212/1200. The left part of the image illustrates the minor, poorly organised, polyaromatic C phase. Le Coustumer et al. (1993), Monthioux and Delverdier (1996) and Laanani (1997). The smallest grains are now about 30–40 nm, many are in the range of ~100 nm, and the largest diameters are difficult to measure by TEM due to the chances of overlapping for crystals whose large dimensions make them no longer electron transparent. In addition, an amorphous oxide layer about 2 nm thick at the grain surface is still found, quite similar to that of Figure 4.8. Nevertheless, the C phase associated to SiC crystals is also still found, though less abundant, with about the same textural and structural features than that found in Figures 4.2 or 4.6. Electron diffraction patterns show that β is the most frequent SiC structure, but the occurrence of
< previous page
page_60
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_60.html [20/01/2010 10:03:37 AM]
page_61
< previous page
page_61
next page >
Page 61 diffraction spots located besides the regular 111, 200, 220 and 311 diffraction rings for the 3C polytype indicates that other polytypes (α structures) are present (Figure 4.10). SIC173, 1800°C ANNEALED The main effect of such a high heat-treatment temperature is the development of the polyaromatic C phase, either as SiC-free porous material or shells around SiC crystals (Figure 4.11). Though still turbostratic as ascertained by electron diffraction patterns, since only 00l reflections and hk bands are present (Figure 4.12 (a)), the nanotextural state of the C phase is very good, that is, exhibiting perfect graphene stacks at long range (Figure 4.13), which is consistent with a probable origin from the partial SiC decomposition (Oberlin et al. 1976; Iijima
Figure 4.10 Electron diffraction of the SiC phase from SiC177/1500. The 3C (β structure) polytype is prevalent, but some other polytypes are found.
Figure 4.11 TEM bright-field image from SiC173/1800. The partial decomposition of SiC crystals induces the secondary formation of empty or crystal-filled C shells.
< previous page
page_61
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_61.html [20/01/2010 10:03:38 AM]
page_62
< previous page
page_62
next page >
Page 62
Figure 4.12 Electron diffraction patterns from SiC173/1800. (a) On the C phase: the structure is turbostratic, since only hk reflections are found in addition to the 002 reflection. (b) On SiC crystals (+C). The 3C polytype of SiC is no longer prevalent.
Figure 4.13 TEM lattice fringe image from SiC173/1800. Walls of the C shells seen edge-on. The nanotexture (i.e. graphene perfection) is very good, though the structure is not graphitic but turbostratic according to electron diffraction patterns. 1982). Indeed, though the decomposition of SiC might sound doubtful since 1800°C is still early regarding the theoretical sublimation temperature of SiC (2700°C), the SiC crystals are the only C source available to explain the increase in the C phase amount. Beside, the average SiC grain size increased dramatically (more than two to four times larger than in the starting material), which is consistent with the similar effect observed in the SiC177/1500°C sample (but in a lesser extent). Meanwhile, the diffraction patterns now exhibit many diffraction spots other than that of the 3C polytype, indicating the occurrence of other polytypes (Figure 4.12(b) as compared to Figure 4.3).
< previous page
page_62
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_62.html [20/01/2010 10:03:39 AM]
page_63
< previous page
page_63
next page >
Page 63 SIC173, 450°C OXIDISED As a result of the oxidising treatment, the daylight colour of the powder has turned from dark grey to greengrey. The treatment was successful in removing the primary polyaromatic C phase without altering the SiC grains (Figure 4.14), as compared to the non-oxidised, as-prepared powder (Figure 4.15). Every other feature was kept unchanged. SIC173, 450°C OXIDISED, 1800°C ANNEALED A secondary polyaromatic C phase has appeared again, abundant, as C shells systematically surrounding the SiC grains (see Figure 4.11 for reference). This experiment definitely ascertains that SiC crystals start to decompose at temperatures as low as 1800°C (but beyond
Figure 4.14 TEM bright-field image from SiC173/450—O2. The oxidation treatment was successful in removing the C phase without oxidising the SiC crystals.
Figure 4.15 TEM bright-field image from SiC173. Arrows show the polyaromatic C phase associated to the SiC crystals. To be compared with Figure 4.16.
< previous page
page_63
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_63.html [20/01/2010 10:03:40 AM]
page_64
< previous page
page_64
next page >
Page 64 1500°C, as shown by the 1500°C annealing experiment of sample SiC177, where only the primary C phase was found), although the average grain diameter increases. The fact that this temperature is far below the theoretical sublimation temperature for SiC (2700°C) may be explained by the small sizes of the SiC grains. Generally speaking, physical constants of a given phase are likely to be lowered when finely partitioned into nanocrystals as compared to macrocrystals, due to a higher contribution of surface atoms relative to core atoms (Buffat and Borel 1976). SIC212, 1200°C ANNEALED, 450°C OXIDISED Like for sample SiC173, the daylight colour of the sample has turned from dark grey to green-grey. This is the only change observable. Specifically, the amorphous coating on the SiC grains is still found (not illustrated), ascertaining that the coating is silicon oxide, since amorphous C should have burnt into CO2 during the oxidation experiment. Si/C/N-based powders Two materials were investigated as-prepared, labelled SiCN29 and SiCN35. Related preparation conditions and elemental analysis of the as-prepared materials are reported in Tables 2.2 and 2.3, respectively. Though the amount of silane is similar, they mainly differ from each other both by the amount of nitrogen (N) supplied (twice for the former), and the N-containing gaseous precursors used (CH3NH2 only for the latter, as compared to CH3NH2 + NH3 for the former). This induces a higher supply in C for SiCN35. SICN29, AS-FORMED Daylight colour of the material is light grey-green. As often, the sample exhibits two kinds of morphologies. The major phase is made of large grains, in the range of 20–150 nm, with frequent round shapes (Figure 4.16), sometimes polyhedral (Figure 4.17). According to the
Figure 4.16 TEM bright-field image from SiCN29.
< previous page
page_64
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_64.html [20/01/2010 10:03:41 AM]
page_65
< previous page
page_65
next page >
Page 65
Figure 4.17 Low magnification TEM lattice fringe image of some crystals from SiCN29. dark-field images, each grain is a single crystal (Figure 4.18(b)). Grains are associated to each other into aggregates or chains both by covalent bonding, since lattice fringe imaging suggests structural continuity between adjacent crystals through grain boundaries (Figure 4.19), or by weak forces. They are identified as α-Si3N4 crystals by electron diffraction (Figure 4.20), as supported by the occurrence of the specific reflection 101 at 0.432 nm. However, the concomitant occurrence of the β structure is possible. Indeed, from the point of view of selected area electron diffraction mode, diffraction patterns from α- and β-Si3N4 structures are difficult to distinguish from each other, due to the high amount of reflections many of which are present in both structures on one hand, and due to the frequent absence of either complete diffraction patterns or complete diffraction rings on the other hand. Although lattice fringe images reveal some distorted fringes at the Si3N4 crystal surface looking like turbostratic C stacks (Figure 4.19), it is believed that, unlike in the SiC-based powders, they do not correspond to a polyaromatic C phase. Indeed, the X-EDS spectra (Figure 4.21) do not show any presence of C (either sp2 or sp3), neither associated to the Si3N4 major phase nor to the SiOxNy minor phase (see below). Also, considering the chemical balance for a SiC-based sample like SiC173 (Table 2.3) shows that 2 wt% only of calculated excess C are enough to provide obvious evidence of polyaromatic C stacks in the lattice fringe or dark-field images (Figures 4.2 or 4.5(a) and (b), respectively). On the contrary, twice a calculated amount of excess C in SiCN29 would barely correspond to the few distorted stacks (in lattice fringe mode, Figure 4.19) or bright rims (in dark-field mode, Figure 4.18(a), open arrow) shown in the TEM images. The absence of a polyaromatic C phase is therefore suggested, and the phase found at the crystal surface is more likely a silicon oxinitride phase. Actually, previous studies combining both TEM and XPS investigations and performed on various Si3N4 powders have shown that silicon oxinitride is able to exhibit the same kind of distorted fringes as turbostratic C (Madigou et al. 1990a, b; Madigou 1991). However, since the chemical balance indicates the presence of C atoms, they could possibly be incorporated into the amorphous silicon oxinitride phase with such a low proportion that would make C non-detectable. Such amorphous silicon oxicarbonitride phases do actually exist, as synthesised from the thermal curing under gaseous oxygen or air of polycarbosilazane polymers (Okamura et al. 1984; Mocaer et al. 1993).
< previous page
page_65
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_65.html [20/01/2010 10:03:42 AM]
page_66
< previous page
page_66
next page >
Page 66
Figure 4.18 TEM dark-field image sequence from SiCN29. (a) ‘C-specific’ (DF1) imaging conditions. Actually, crystals appearing bright are not C but Si3N4 crystals. They are imaged in the selected imaging conditions because the crystals exhibit lattice distances close to that of C002. Likewise, the white arrow shows bright rims which are more likely an organised Si—O—N phase rather than a polyaromatic phase, according to XEDS spectra (see text). The black arrow shows a polyaromatic C-rich phase. (b) ‘SiC-specific’ (DF2) imaging conditions. Crystals appearing bright are actually not SiC but Si3N4. They are imaged in the selected imaging conditions because the crystals exhibit lattice distances close to that of SiC111. The fact that the crystals are thus able to be imaged in both dark-field imaging conditions allow them to be identified as Si3N4 instead of C or SiC.
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_66.html (1 of 2) [20/01/2010 10:03:43 AM]
page_66
Figure 4.19 TEM lattice fringe image on Si3N4 crystals from SiCN29. Evidence of a coating layer, ~1 nm thick, at the crystal surface, whose distorted fringes are oriented parallel to the grain surface.
< previous page
page_66
next page >
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_66.html (2 of 2) [20/01/2010 10:03:43 AM]
page_67
< previous page
page_67
next page >
Page 67
Figure 4.20 Electron diffraction from SiCN29. Si3N4 crystals typically exhibit a lot of lattice distances at small scattering angles.
Figure 4.21 X-EDS spectrum on some Si3N4 crystals from SiCN29. The occurrence of O and the absence of C suggests that the phase coating the crystals is actually Si—O—N-type. The minor phase is made of grains whose size range is often lower than for the major phase, with round shapes. Since always faintly scattering the electron beam in dark-field imaging mode whatever the position of the objective aperture (Figures 4.18(a) and (b)) – though decreasingly as the tilt angle increases – the structure of this phase is amorphous. The chemical composition is qualitatively given by X-EDS measurements (not illustrated), which indicate an enrichment in oxygen and a depletion in N relative to the Si3N4 phase (Figure 4.21), in addition to the presence of Si. It is therefore believed that this minor phase is amorphous silicon oxinitride or oxicarbonitride.
< previous page
page_67
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_67.html [20/01/2010 10:03:43 AM]
page_68
< previous page
page_68
next page >
Page 68 SICN35, AS-FORMED Daylight colour of the material is dark grey-green. As sample SiCN29, two morphologies are again observed. The major phase exhibits large grains with irregular and polyhedral shapes associated into compact aggregates (Figure 4.22). Size range cannot be ascertained due to the superimposition effects which make the grain contours difficult to determine. Dark-field imaging reveals that each grain is itself an aggregate containing crystals with various sizes up to about 40 nm (Figure 4.23(c)). These crystals were identified as pure β-SiC (=3C polytype only) by electron diffraction (Figure 4.24). Both dark-field (Figure 4.23(a)) and lattice fringe (Figure 4.25) images reveal that the SiC crystals are associated with an amorphous phase somewhat embedding them. According to the X-EDS analysis which shows the presence of N and O in addition to Si and C (not illustrated), this amorphous phase is probably a silicon oxinitride or oxicarbonitride. No turbostratic C phase was revealed. The minor phase exhibits much smaller grain sizes, in the range of 10–30 nm, with round shapes, associated into elongated chains (Figure 4.22, arrow). Dark-field imaging (Figure 4.23(b), arrow) supported by lattice fringe imaging (Figure 4.26) both reveal that each grain is itself an aggregate of tiny crystals, few nanometres large. They were identified as Si crystals (CFC structure) by means of electron diffraction (Figure 4.27). Correspondingly, lattice fringe images show lattice distances consistent with the (111) planes of Si (Figure 4.26). These images also reveal that Si crystals are associated with an amorphous phase, located at their outer surface as a coating, about 2 nm thick (Figure 4.26). According to the X-EDS analysis which barely shows another light element than O (in addition to the prevalent Si peak – not illustrated), this amorphous phase is probably a silicon oxide phase, which is likely considering the sensitivity of pure Si to oxidation.
Figure 4.22 TEM bright-field image from SiCN35. Arrows show chain-like aggregate of small grains.
< previous page
page_68
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_68.html [20/01/2010 10:03:44 AM]
page_69
< previous page
page_69
next page >
Page 69
Figure 4.23 TEM dark-field image sequence from SiCN35. (a) ‘C-specific’ (DF1) imaging conditions. No crystals appear, indicating that no Si3N4 crystals are present (see Figure 4.20 caption for further explanation). (b) Dark-field imaging conditions selected are intermediate between (a) and (c), therefore admitting both C002 and SiC111 distances. Both SiC crystals and another phase (arrowed) are imaged. (c) ‘SiC-specific’ (DF2) imaging conditions. The azimuthal angle is same as for (b). Correspondingly, the same SiC crystals as in (b) are imaged, but the crystals arrowed in (b) no longer appear, attesting that they are not SiC, but Si crystals (see Figures 4.26 and 4.27).
Figure 4.24 Electron diffraction on a SiC-rich area from SiCN35. Crystals are pure β-SiC crystals.
< previous page
page_69
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_69.html [20/01/2010 10:03:45 AM]
page_70
< previous page
page_70
next page >
Page 70
Figure 4.25 TEM lattice fringe image from the SiC phase from SiCN35. SiC crystals are embedded in an amorphous phase.
Figure 4.26 TEM lattice fringe image from the Si phase from SiCN35. Si crystals are coated with an ~1–2 nm thick amorphous phase, very probably silica. Conclusion regarding ceramic nanopowders from gaseous precursors SI/C-BASED MATERIALS Though SiC173 was the only material investigated as-prepared, it is believed that comparing SiC173 with SiC177/1200 and SiC212/1200 is possible since the annealing temperature is rather low. Since the ethylene/ silane ratio is about the same (~0.5) for all the samples, the main difference in preparation conditions lies in the total flow rate. It increases from SiC177 to SiC173 to SiC212 for a similar C/Si ratio in the precursor gases, inducing a decrease in the residence time from 12.1 to 7.3 then 2.5 ms, respectively (Table 2.2). Correspondingly,
< previous page
page_70
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_70.html [20/01/2010 10:03:46 AM]
page_71
< previous page
page_71
next page >
Page 71
Figure 4.27 Electron diffraction on a Si phase-rich area from SiCN35. Crystals are pure Si, CFC structure. the grain size range decreases, and SiC polytypes other than the primary form 3C (β structure), though present in the two former samples, do not have the time to develop in the latter. Likewise, the organisation of the polyaromatic C phase tends to decrease. Conditions for the preparation of SiC212 prevent the occurrence of a primary polyaromatic C phase. One explanation could be that long residence times used for SiC173 and SiC177 allow a Si—C—(H) solid solution enriched in C (relative to the 1:1 stoichiometry of SiC) to form in the reaction zone. The subsequent crystallisation of the SiC phase makes the excess C to be expelled as a polyaromatic C phase associated to the SiC crystals. Heat treatments in inert atmosphere provoke the increase in the average SiC grain size due to a coalescence mechanism (i.e. growth from coalescence) by impingements, while the primary C phase, when any, remains unchanged up to 1500°C. Beyond 1500°C (at least from 1800°C), the latter mechanism competes with an early decomposition mechanism, due to the nanometric size of the SiC phase. The partial decomposition of SiC induces the formation of a secondary polyaromatic C phase. Meanwhile, the SiC structure tends to increasingly change from a majority of 3C (cubic) polytype to a mixture of various polytypes (except 2H which is irreversibly unstable beyond ~1600°C – Inoue and Kourachi 1983), probably mostly as stacking fault sequences within the same grains. An explanation is that the coalescence mechanism involves solid crystals, that does not allow single crystals with defect-free, homogeneous structure to be obtained. SI/C/N-BASED MATERIALS Correspondingly to the higher N content in the precursor gas phase for SiCN29 (twice that of SiCN35), Si3N4 crystals only develop in the former. A SiC phase develops in SiCN35 instead, further enhanced by a higher amount of C supply. The fact that no Si3N4 phase is able to form in SiCN35 is amazing since, consistently with the theoretical phase content calculated from the elemental composition (Table 2.3), the N supply should be sufficient. This is not merely due to a lower formation kinetic for Si3N4 relative to SiC, since Si3N4 is able to form in SiCN29 while the residence time is lower. The main parameter is therefore believed to be the nature of the primary gases, and possibly the presence of C specifically.
< previous page
page_71
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_71.html [20/01/2010 10:03:47 AM]
page_72
< previous page
page_72
next page >
Page 72 Thus, when combined with silane and ethylene, a C-free precursor like NH3 is more likely to induce the Si3N4 formation than a C-containing precursor like CH3NH2. The reason is probably that the former precursor gas combination only provides C—H, Si—H and N—H bonds which are easier to thermally break than the preexisting C—N bonds in the latter. Si N bonds are therefore allowed to form more easily and early in the former than in the latter. 4.1.2 Synthesis from liquid precursors Nebulisation of liquid precursors such as hexamethyldisilazane (Si2C6NH18) produced other Si/C/N-based powders. Adding an increasing amount of NH3 allowed the C/N atomic ratio of the as-prepared material to be controlled. The various experiments result in a whole series of samples listed in Table 2.5, and characterised by a continuous decrease in their C/N atomic ratio. On the other hand, the same principle of using an increasing NH3/Ar ratio for a constant total flow rate was applied to a nebulised liquid precursor made of a mixture of HMDS and aluminium isopropoxide (see Section 2.4.2) in order to prepare Si/Al/C/N-based powders. Materials obtained and relative preparation conditions are reported in Table 2.6. Si/C/N-based powders Among the whole series of samples listed in Table 2.5, HMDS42 and HMDS44 were investigated by TEM. They correspond to a slope change in the variation trend of the C/N ratio value measured in the starting materials v. the SiC/Si3N4 content in the 1600°C-annealed materials (see Figure 3.9). HMDS42 and HMDS44 exhibit C/N ratios of 0.73 and 0.56, respectively. Since amorphous at the as-prepared state, they were investigated after increasing annealing heat treatments under pure N atmosphere at temperatures ranging from 1000°C to 1600°C. HMDS42, 1000°C ANNEALED The bulk structural evolution of the sample with increasing annealing temperature from 1000°C and beyond is illustrated by electron diffraction, whose patterns are gathered on Figure 4.28. After 1000°C annealing, the daylight colour of the material is black. Though all the grains exhibit a rather round and isometric morphology (Figure 4.29(a)), a two-mode distribution of grain size is observed, with small grains (20–60 nm) being prevalent, and the subsidiary occurrence of large grains (80–60 nm). Small grains exhibit a nanometric porosity revealed by a Fresnel contrast effect when unfocused. Grains are associated into aggregates (often chain-like) either by strong, structural bonds (illustrated by the chain-like aggregate made of three large grains at the centre of Figure 4.29(a)), or by weak (electrostatic) forces (as illustrated by the small grain aggregate at the top of Figure 4.29(a)). It is worth noting that isolated grains look isometric, but aggregates are not. Considering one morphology (isometric) or the other (chain-like for instance) will provide very different shape factors, which is likely to explain possible mismatches between actual and calculated surface area of the powder. Electron diffraction patterns indicate an overall amorphous structural state, both for large and small grains (Figures 4.28(a) and (b)). However, patterns from small grains exhibit an additional modulation (white arrow) whose location suggests the early occurrence of
< previous page
page_72
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_72.html [20/01/2010 10:03:47 AM]
page_73
< previous page
page_73
next page >
Page 73
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_73.html (1 of 2) [20/01/2010 10:03:48 AM]
page_73
Figure 4.28 Electron diffraction from HMDS42 on large grain and small grain phases respectively after increasing annealing treatment. From (a) to (g) the arrows show the occurrence of a faint C002 reflection.
< previous page
page_73
next page >
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_73.html (2 of 2) [20/01/2010 10:03:48 AM]
page_74
< previous page
page_74
next page >
Page 74
Figure 4.29 TEM bright-field image and dark-field image sequence from HMDS42/1000. (a) illustrates the differentiation into two phases with different grain size range. (b) ‘C-specific’ dark-field imaging conditions. The polyaromatic C phase appears as tiny bright dots representing primary graphene stack entities ~1 nm large. (c) ‘SiC-specific’ dark-field conditions. No phase has crystallised yet. very small (<1 nm) C (polyaromatic) entities. The stacking distance (~0.37 nm) is larger than for usual turbostratic C (0.344 nm) but similar to that found in immature organic precursors (Oberlin et al. 1980, 1986). These nanometric C entities are expected to appear as small bright dots in C-specific dark-field imaging mode (see Annexe) as illustrated in Figure 4.29(b). However, due to the limited resolution in darkfield imaging conditions (δ ~ 0.7 nm), bright dots from the small polyaromatic entities cannot be distinguished from the background of dots originating from each atom pairs from the surrounding amorphous material. No other crystallised, nanometric phase like SiC is found, since SiC-specific dark-field images only exhibit the regular scattered intensity of amorphous material (Figure 4.29(c)). A polyaromatic C phase is, therefore, present in the small grains, whose graphenes are at the very beginning of their face-to-face association (Monthioux 1998). This should probably be related to the nanoporous texture of the grains. Otherwise, no other difference is detected between large and small grains, which exhibit the same bulk chemical composition, with the respective X-EDS spectra similar to that of Figure 4.21, however with a higher contribution of C. HMDS42, 1300°C ANNEALED Important structural changes occur in both grain types. The modulation attributed to the 002 reflection of a polyaromatic, turbostratic C phase in small grains becomes stronger in diffraction patterns (Figure 4.28(c), white arrow). The C phase is now evidenced at the grain
< previous page
page_74
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_74.html [20/01/2010 10:03:49 AM]
page_75
< previous page
page_75
next page >
Page 75 surface, where it now appears as bright rims in dark-field images (Figure 4.30(a)), and as small fringe stacks in high-resolution images, mostly oriented parallel to the grain surface, either at small grain surface (Figure 4.31) or large grain surface (though C is systematically less abundant than for small grains, not illustrated). Such a preferred occurrence of the polyaromatic stacks at the grain surface in C-rich amorphous ceramics with increasing annealing temperature is a common observation (Monthioux et al. 1990; Delverdier et al. 1992a,b, 1993, 1994). It is probably due to easier atomic movements at the grain surface, allowing C segregation on one hand and a graphene display more or less parallel to the grain surface on the other hand. The proportion of the C phase is obviously much higher in small grains than in large grains. It is still poorly organised, since it is made of distorted graphenes about 1–2 nm wide (L2) only, stacked by N = 2–4 only. Also, the occurrence of some brighter dots irregularly disseminated in SiC-specific dark-field images (Figure 4.30(b)) indicates the very beginning of crystallised SiC-phase segregation as nanometric crystals, possibly clusters. Such an early crystallisation step was hardly guessed from the related diffraction patterns (Figures 4.28(c) and (d)) due, on one hand to the relative amount of scattering volumes for the amorphous and the crystallising parts of the material respectively, on the other hand to the overlapping of the SiC reflections, which are very faint and broad as a consequence of the tiny sizes of the SiC crystals involved.
Figure 4.30 TEM dark-field image sequence from HMDS42/1300. (a) ‘C-specific’ (DF1) imaging conditions. Graphene stack entities parallel to the ‘=’ sign are selected, showing that they tend to align parallel to the grain surface. (b) ‘SiC-specific’ (DF2) imaging conditions. Nanometric dots appear, indicating the early stage of overall SiC nucleation.
< previous page
page_75
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_75.html [20/01/2010 10:03:50 AM]
page_76
< previous page
page_76
next page >
Page 76
Figure 4.31 TEM lattice fringe image from HMDS42/1300 (small grains). Poorly organised graphene stacks at the grain surface are imaged. HMDS42, 1400°C ANNEALED Same features as above (Figure 4.28(e)), but the occurrence of the C phase becomes higher and higher, while its organisation improves, mainly by increasing L2 more than increasing N (not illustrated). HMDS42, 1500°C ANNEALED In both small and large grains, the overall crystallisation of a β-SiC phase is now obvious, as revealed by the evidence of an intense, though broad, 111 reflection (black arrow in diffraction patterns, Figures 4.28(f) and (g) for small and large grains, respectively). Crystal sizes are still very small, nanometric, inducing wide reflections so that 220 and 311 overlap. This is verified in SiC-specific dark-field images, where crystals as large as ~5 nm are very seldom, most of them being in the 1 nm range (Figure 4.32(b)). It is worth noting that the 002 reflection of the turbostratic C phase, now close to 0.344 nm, still appears for small grains only (Figure 4.28(f)). The C phase is now obviously present at the small grain surface and possibly within them (Figure 4.32(a)). It is responsible for an apparent nanometric porosity (Figure 4.33). High-resolution images illustrate the improvement in the abundance and organisation of the polyaromatic C phase associated with small (Figure 4.34) and large (see Figure 4.19 as reference for the abundance and organisation of the surface C exclusively) grains, respectively. Compared to the chemical composition of the grains in the material annealed at 1000°Cas seen by X-EDS(see Figure 4.21 for reference), the chemical composition given by X-EDS analysis of the 1500°C-annealed material reveals a depletion in oxygen content indicated by a lower O/N ratio in both small and large grains (Figure 4.35). This suggests that oxygen atoms were initially not involved in SiO4 tetrahedra from silica since the latter is stable at 1500°C, but possibly in SiOxCyNz tetrahedra similar to that formed in polymer-derived Si/C/N-based ceramics (Delverdier et al. 1994). This is consistent with the fact that no other crystallised phase but polyaromatic C and SiC is evidenced, indicating the necessary occurrence of an amorphous silicon oxi(carbo)nitride phase as an intergranular phase between
< previous page
page_76
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_76.html [20/01/2010 10:03:51 AM]
page_77
< previous page
page_77
next page >
Page 77
Figure 4.32 TEM dark-field image sequence from HMDS42/1500 (small grains). (a) ‘C-specific’ (DF1) imaging conditions. As the contrast between the bright dots and the background increases, the organisation of the graphene stacks improves. (b) ‘SiC-specific’ (DF2) imaging conditions. SiC growth has started.
Figure 4.33 TEM bright-field image from HMDS42/1500 (small grains). The development of the C phase provides a textured aspect to the grains. Superimposition effects of the projected image do not allow to ascertain whether most of the C is inside or outside the grains.
< previous page
page_77
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_77.html [20/01/2010 10:03:52 AM]
page_78
< previous page
page_78
next page >
Page 78
Figure 4.34 TEM lattice fringe image from HMDS42/1500 (small grains), illustrating the improvement of the polyaromatic C phase organisation and development with temperature (compare with Figure 4.31).
Figure 4.35 X-EDS spectrum from HMDS42/1500. Valid for large or small grain phases. SiC grains. The partial removal of oxygen atoms from this amorphous phase due to the annealing temperature should probably be related to the crystallisation of the SiC phase, as a cause or a consequence of it for thermodynamic reasons. HMDS44, 1400°C ANNEALED As determined by means of electron diffraction, dark-field, bright-field, and lattice fringe imaging modes, its features are very similar to that of sample HMDS42 annealed at the same
< previous page
page_78
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_78.html [20/01/2010 10:03:53 AM]
page_79
< previous page
page_79
next page >
Page 79
Figure 4.36 TEM bright-field image from HMDS44/1400. The extensive development of a polyaromatic C phase at the grain surface is obvious. temperature, and will therefore not be extensively illustrated again. However, one discrepancy is a slightly smaller grain size range, that is, 20–50 nm. Another is that crystallisation of SiC phase has not even started yet. The average polyaromatic C content is difficult to estimate since the material appears again heterogeneous, with both grains associated with an abundant C phase (Figure 4.36), and grains associated with few C phase (see Figure 4.19 as reference for the abundance and organisation of the surface C) or none. At least, there is no obvious contradiction with the result from the bulk elemental analysis, which reveals a continuous decrease in the C content from sample HMDS40 to HMDS45 (Table 2.5). Qualitatively, it is worth noting that the occurrence of polyaromatic C is also ascertained by other investigation methods like electron spin resonance (ESR) and X-photon spectroscopy (XPS) (Chapters 5.2 and 5.3). HMDS44, 1500°C ANNEALED Features are identical to that of the 1400°C-annealed sample described above. The interesting observation is that, contrarily to what happened in sample HMDS42 in which a widespread β-SiC phase is found after annealing at this temperature, no crystallisation of a Si-based phase has occurred yet. The bulk material is still amorphous, and still contains Si, C and N, as identified by electron energy loss spectroscopy (EELS) (Figure 4.37). It is worth noting that no oxygen is detected. An extended EELS study in a VG STEM microscope was specifically performed by N. Brun (Laboratoire de Physique du Solide, Paris, France) on some grains from this sample in order to tentatively characterise further the C content, using a very fine electron probe combined with scanning facility. Quantitative exploitation of the EELS spectra led to a bulk
< previous page
page_79
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_79.html [20/01/2010 10:03:54 AM]
page_80
< previous page
page_80
next page >
Page 80
Figure 4.37 EELS spectrum (large probe) from HMDS44/1500. Si, C and N are revealed. atomic C content estimated at ~16–20%, most of it being segregated at the grain surface (Figure 4.38(a)) as sp2 C atoms, that is, as a polyaromatic C phase (Figure 4.38(b)). On the contrary, the grain core was found to contain ~4% of sp2-type C atoms (Figure 4.38(b)), giving an inner C/N atomic ratio of ~0.2 (together with an inner N/Si atomic ratio of ~1.3). All these values strongly support the previous observations on the C phase occurrence, type and location, and are fairly consistent with the quantitative data obtained otherwise. In addition, the Si amount in the bulk is more that twice that of the C amount corresponding to the sum of the inner and outer C (Figure 4.38(a)). This and the occurrence of an abundant N content (~45%) show that an Si—(C)—N amorphous phase is also present in the grain in addition to the SiC crystals. HMDS44, 1550°C ANNEALED The SiC phase crystallises first, exhibiting peculiar polyhedral morphologies, most often triangular (sometimes rectangular) corresponding to the primary crystalline form of the cubic (hemihedral) structure of SiC (Figure 4.39). HMDS44, 1600°C ANNEALED Overall crystallisation of both Si3N4 and SiC has occurred. It is likely that the location where Si3N4 and SiC phases crystallise is correlated to the previous occurrence of polyaromatic-carbon-depleted and polyaromaticcarbon-rich grains, respectively. Grain sizes are in the 50–200 nm range (Figure 4.39). Electron diffraction shows that the cubic (3C) structure is probably no longer prevalent, and a lot of other polytypes are found since additional diffraction spots other than 111, 200, 220 and 311 of β-SiC are present, often as stacking faults as indicated by the specific occurrence of aligned spots (Figure 4.40, arrow). The triangular shape of the SiC crystal projection suggests that the growth has occurred in conditions of saturation (i.e. no limitation in the C and Si atom supply) or, at least, in conditions such that feeding atoms have equal access opportunity to the various crystal faces, since the relative growth speeds of the various faces were respected. In such conditions, ‘slow’ faces (like (111)) are actually favoured relative to ‘fast’ faces (like (100)) since the latter require less atoms than the former to be completed.
< previous page
page_80
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_80.html [20/01/2010 10:03:54 AM]
page_81
< previous page
page_81
next page >
Page 81
Figure 4.38 Data obtained from scanning nanoprobe EELS performed on single grains from HMDS44/1500. (a) EELS quantification of Si, C and N (in at% along y axis) within half a grain (grain radius along x axis) showing that most of the C content is at the grain surface. (b) sp2 (solid symbols) and sp3 (open symbols) C atom content quantification within a grain about 50 nm large, indicating that the surface C is exclusively polyaromatic (sp2). Data from N. Brun, Laboratoire de Physique du Solide, Paris, France.
< previous page
page_81
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_81.html [20/01/2010 10:03:55 AM]
page_82
< previous page
page_82
next page >
Page 82
Figure 4.39 TEM bright-field image from HMDS42/1600 (SiC phase). Most of the SiC crystals exhibit a triangular projection.
Figure 4.40 Electron diffraction from HMDS42/1600 (SiC phase). A lot of polytypes other than 3C are present, including as stacking faults (arrows). On the other hand, the Si3N4 phase was not investigated, due to the very large size range of the crystals (several micrometers) making them not transparent to the TEM electron probe. However, crystallised Si3N4 was otherwise undoubtedly revealed by X-ray diffraction (XRD).
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_82.html (1 of 2) [20/01/2010 10:03:56 AM]
page_82
< previous page
page_82
next page >
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_82.html (2 of 2) [20/01/2010 10:03:56 AM]
page_83
< previous page
page_83
next page >
Page 83 Finally, it is worth noting that the polyaromatic C phase is no longer found, suggesting an oxidation into CO (rather than CO2, because of the high temperature) due to the release of oxygen consequently to the crystallisation of SiC and Si3N4. Si/C/N/Al-based powders Among the various samples prepared following this route, three were specifically investigated by TEM, asprepared first, then after a 1600°C (1 h isothermal) annealing under N atmosphere. Samples labelled HSAl07, HSAl12 and HSAl09 thus respectively correspond to 0/100, 20/80 and 40/60 NH3/Ar proportions in the gas phase. HSAL07, AS-FORMED The colour of the macroscopic powder at natural light is grey. In TEM, electron diffraction shows that the bulk sample is amorphous (Figure 4.41). Grain size range from ~20 to ~130 nm, with a tendency to a twomode distribution (Figure 4.42). The overall grain morphology is round, although the smallest grains may tend to be more or less slightly polyhedral. Another difference between small (i.e. in the range ~20–60 nm) and large grains (i.e. in the range 50–130 nm) is that the former exhibit some nanometric porosity (Figure 4.43), suggesting some primary difference in chemical composition. No polyaromatic C phase was revealed at the grain surface either by means of dark-field (not illustrated) or lattice fringe imaging (Figure 4.44). However, some primary, nanometric graphene stack entities are possibly imaged (Figure 4.44, arrows). Also, some poorly organised polyaromatic C particle (~15–30 nm) aggregates similar to C blacks (not illustrated) were found as a seldom phase apart from the amorphous phase. HSAL12, AS-FORMED The natural light colour of the macroscopic powder is black. The material differs from HSAl07 by the grain size range, which is more obviously shared into two sub-size ranges
Figure 4.41 Electron diffraction from HSAl07. The whole material is amorphous.
< previous page
page_83
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_83.html [20/01/2010 10:03:56 AM]
page_84
< previous page
page_84
next page >
Page 84
Figure 4.42 TEM bright-field image from HSAl07. The two-mode grain size distribution is shown.
Figure 4.43 High magnification TEM bright-field image from HSAl07. Small grains (bottom) exhibit a nanotexture while large grains (top) do not. (see Figure 4.42 for reference). The most prevalent one is ~10–30 nm, whose grains are more or less polyhedral and exhibit a nanometric porosity (see Figure 4.43 for reference). The minor one is ~50–100 nm, with grains having round contours and no obvious porosity. The main difference with HSAl07 is that the early crystallisation of a widespread, poorly organised, turbostratic, polyaromatic phase is suggested by a faint C002 halo in electron diffraction patterns (Figure 4.45, arrow), further supported by the occurrence of tiny brighter
< previous page
page_84
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_84.html [20/01/2010 10:03:57 AM]
page_85
< previous page
page_85
next page >
Page 85
Figure 4.44 TEM lattice fringe image from HSAl07. Primary nanometric graphene stacks are probably showed.
Figure 4.45 Electron diffraction from HSAl12. The whole material seems amorphous. spots into the grains and some bright rims at the grain surface in the related dark-field images (Figure 4.46, arrow). Likewise, the early crystallisation of SiC has also started in the small grains, as revealed by the SiC-specific dark-field images (left side in Figure 4.47, arrows) while large grains remain amorphous (right side in Figure 4.47). Indeed, the fact that no such crystals appear in ‘C-specific’ dark-field images (Figure 4.46) ascertain that crystals are actually SiC, not Si3N4 (see Section 4.3). It is worth noting that, unlike what was found for SiCxxx- or HMDSxx-type materials, the SiC crystallisation does not start according to an overall, widespread germination mechanism resulting in a homogeneous dissemination of nanometric crystals in
< previous page
page_85
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_85.html [20/01/2010 10:03:58 AM]
page_86
< previous page
page_86
next page >
Page 86
Figure 4.46 TEM dark-field image from HSAl12. ‘C-specific’ (DF1) imaging conditions. Bright dots within small grains and bright rims at grain surface appear, indicating the occurrence of a poorly organised, polyaromatic C phase. the material, but rather corresponds to the local occurrence of the appropriate nucleation-then-growth conditions, resulting in the random but seldom occurrence of SiC crystals. The amount of crystals is not enough to appear in the diffraction patterns (Figure 4.45), but the β structure can be ascertained from the dark-field data. HSAL09, AS-FORMED The natural light colour of the macroscopic powder is heterogeneous with grey to light brown areas. The overall TEM features of the sample are very similar to HSAl12 regarding the two-class grain size distribution (see Figures 4.42 or 4.47 for reference), the early occurrence of seldom SiC crystals in the small grains, the absence of Si3N4, and the possible occurrence of a widespread, poorly organised, polyaromatic phase. However, the latter is less ascertained since no C rims at the grain surface were found. Some C black type aggregates are also found (not illustrated).
< previous page
page_86
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_86.html [20/01/2010 10:03:59 AM]
page_87
< previous page
page_87
next page >
Page 87
Figure 4.47 TEM dark-field image from HSAl12. ‘SiC-specific’ (DF2) imaging conditions. SiC crystals are found locally in small grains, already several nanometres large. HSAL07, 1600°C ANNEALED The macroscopic natural light colour of the sample has turned from grey to black. The material is quite homogeneous, and a single morphology of round or slightly polyhedral grains was found in TEM images (see Figure 4.22 for close enough reference). The grain size range is ~30 to ~60 nm, therefore, significantly narrower than in the as-prepared materials, which has to be related to some weight loss during the ceramisation process. Appropriate darkfield imaging (not illustrated) shows that each grain is actually an aggregate of round single crystals (~2–25 nm) with a non-symmetrical grain size distribution since a majority of them are less than ~10 nm. Electron diffraction identifies the crystals as SiC with the prevalent β (3C) structure since reflections 111, 220 and 311 are the only ones being revealed as diffraction rings, although some diffraction spots beside these rings appear, showing the seldom occurrence of other polytypes (see Figure 4.8 for reference). Correspondingly, some crystals exhibit stripes in dark-field images, revealing polytype sequence as stacking faults. The association of the SiC crystals into larger grains implies the occurrence of a binder, that is, an intergranular amorphous phase to ensure the grain cohesion, obviously containing N and Al, in addition to some Si and possibly C. A polyaromatic C phase is now revealed at the grain surface (though not systematically), either by dark-field (not illustrated) or lattice fringe imaging (see Figure 4.37 for reference), which is responsible for most of the polyhedral contours of the grains. The cohesion of the aggregates is ensured by an intergranular amorphous phase, that X-ED Sreveals to contain at least Al and O, in addition to probably Si and possibly C. Also, traces of K, Ca and Na are found (Figure 4.48).
< previous page
page_87
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_87.html [20/01/2010 10:04:00 AM]
page_88
< previous page
page_88
next page >
Page 88
Figure 4.48 X-EDS spectrum of the SiC-containing grains from HSAl07/1600. The occurrence of Al and O in addition to Si and C suggests that these elements are present in the composition of an intergranular amorphous phase. No N-containing amorphous or crystallised phases are found, while N is more abundant than O in the material according to the bulk chemical composition (Table 2.6). This emphasises the fact that the qualitative comments about the respective proportions of the various phases are only valid for the material once prepared for TEM investigation. Actually, when a phase is present as very large grains (i.e. micrometric) together with another phase with smaller grains (sub-micrometric), the suspension method used to prepare an electron transparent aliquot of the materials favours the prevalence of the latter relative to the former, with no respect to the original proportions. It is therefore possible that large grains of Si3N4 (or SiAlON) were present in the material, though not found in the TEM preparation. HSAL12, 1600°C ANNEALED The natural light colour of the macroscopic powder has turned from dark to light grey-green. The whole material is crystallised. The SiC phase is the most frequent (in the TEM preparation of the material, see the end remark of previous section) and appears as grains ~20–100 nm large, exhibiting systematic triangular projections (see Figure 4.39 for reference). Electron diffraction shows that the cubic (3C) structure is not prevalent since the related 220 and 311 reflections barely form complete rings in the diffraction patterns (see Figure 4.40 for reference). Many other diffraction spots corresponding to other lattice distances are found instead, therefore, revealing the occurrence of other polytypes. Crystals are frequently coated with an amorphous phase, few nanometres thick (not shown), believed to be different from mere silica since containing at least Al and O (in addition to possibly Si and C) according to X-EDS spectra (see Figure 4.48 for reference), which helps in bonding the crystals to each other (not shown, similar to Figure 4.8). Large, somewhat elongated, micrometric crystals, therefore, not electron transparent, were also found (Figure 4.49). They are free of any amorphous coating, and provide only Si and N with a small contribution of Al and traces of O in X-EDS spectra (Figure 4.50), suggesting a SiAlON-type composition. Other crystals exhibit a needle-like morphology (Figure 4.51). Some observations suggest that they somehow originate from cleavages of the larger, massive
< previous page
page_88
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_88.html [20/01/2010 10:04:00 AM]
page_89
< previous page
page_89
next page >
Page 89
Figure 4.49 TEM bright-field image from HSAl12/1600. Large, dark grains are SiAlON crystals, while needlelike grains are Si3N4 crystals according to X-EDS spectra. Arrow shows that the latter probably originates from the former by cleavages.
Figure 4.50 X-EDS spectrum from large, dark crystals from HSAl12/1600. Al is shown, probably together with O as a shoulder at the right side of the N peak, suggesting a SiAlON composition. crystals (Figure 4.49, arrow). Correspondingly, X-EDS spectra similarly exhibit Si and N, however with the systematic absence of Al and the probable absence of O (Figure 4.52) suggesting that they are genuine Si3N4 crystals, while the needle-like morphology would indicate a structural transformation from α to β. Quantitative mismatches with the phase proportions estimated from XRD (Table 4.1) originate from the segregation effect mentioned at the end of the previous section.
< previous page
page_89
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_89.html [20/01/2010 10:04:01 AM]
page_90
< previous page
page_90
next page >
Page 90
Figure 4.51 TEM bright-field image from HSAl12/1600. Arrow shows that even needle-like crystals are cleaved into smaller needle-like crystals.
Figure 4.52 X-EDS spectrum from needle-like crystals from HSAl12/1600. The absence of Al (and O) indicates a Si3N4 composition. Again, like for material HMDS44/1600, evidence for a polyaromatic C phase was no longer found, suggesting an oxidation into CO (rather than CO2, because of the high temperature) due to the release of oxygen consequently to the crystallisation from the primary O-containing amorphous phase.
< previous page
page_90
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_90.html [20/01/2010 10:04:02 AM]
page_91
< previous page
page_91
next page >
Page 91 Table 4.1 Phase proportions as determined from XRD spectra in 1600°C annealed HSAlxx-type samples Sample reference Results from XRD HSAl07/1600°C β-SiC + α-SiC(ε) HSAl09/1600°C α-Si3N4 + β-Si3N4(ε) HSAl11/1600°C α-Si3N4 + β-Si3N4 HSAl12/1600°C α-Si3N4 + β-Si3N4 + β-SiC HSAl13/1600°C β-SiC + α-SiC HSAl14/1600°C α-Si3N4 + β-Si3N4 + β-SiC HSAl15/1600°C α-Si3N4 + β-Si3N4 + β-SiC HSAl16/1600°C α-Si3N4 + β-Si3N4 HSAl17/1600°C α-Si3N4 + β-SiC + β-Si3N4(ε) HSAl18/1600°C β-SiC + α-SiC Note Underlined = most abundant. (ε) = less than ~5%. HSAL09, 1600°C ANNEALED The natural light colour of the macroscopic powder has turned from light grey-brown to light brown. The same phases (i.e. SiC, and Si3N4 or SiAlON) as in HSAl12/1600 are found, however with different proportions. In addition, some of the primary amorphous phase(s) remain(s), as minor small and large round grains (see Figure 4.42 for reference), whose chemical composition contains Si, N (and O) according to XEDS spectra (not illustrated). The most prevalent morphology is made of aggregates of polyhedral crystals about 20–60 nm large, whose projection are often triangular (Figure 4.53), identified as β-SiC by electron diffraction (Figure 4.54). Some but few polytypes are also present. This SiC phase is associated with an amorphous phase coating the crystals and somewhat acting as an intergranular phase and ensuring the aggregate cohesion. As for the other HSAlxx materials investigated though with various element proportions, the chemical composition of the amorphous phase at least includes Al and O, in addition to possibly Si and C according to X-EDS spectra (see Figure 4.48 for reference). Massive, large, therefore, non-transparent crystals are also found as in material HSAl12/1600 (see Figure 4.49 for reference). A difference is that the morphological transformation into needle-like crystals has barely occurred yet (Figure 4.55) and the latter are seldom, possibly indicating that the α to β transformation has just started. Another difference is that either massive or needle-like crystals exhibit Al and O in addition to Si and N according to X-EDS spectra (Figure 4.56) suggesting a SiAlON-type composition. Mismatches with the phase composition estimated from X-rays originate from the sample preparation for TEM investigation. Conclusion regarding ceramic nanopowders from liquid precursors SI/C/N-BASED MATERIALS Due to their high hydrogen content which makes the materials behave like Si-based polymer-derived ceramics, the as-prepared materials remain mainly amorphous up to annealing temperatures as high as ~1500°C. Such a thermal stability is induced by the complexity
< previous page
page_91
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_91.html [20/01/2010 10:04:02 AM]
page_92
< previous page
page_92
next page >
Page 92
Figure 4.53 TEM dark-field image (‘SiC-specific’ (DF2) imaging conditions) from HSAl09/1600. Many of the crystals exhibit a triangular projection.
Figure 4.54 Electron diffraction from the SiC phase from HSAl09/1600. The 3C polytype is highly prevalent.
< previous page
page_92
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_92.html [20/01/2010 10:04:03 AM]
page_93
< previous page
page_93
next page >
Page 93
Figure 4.55 TEM bright-field image from HSAl09/1600. Large, dark grains are SIALON crystals according to XEDS spectra.
Figure 4.56 X-EDS spectrum from large crystals from HSAl09/1600 (also valid for the needle-like crystals). The occurrence of Al and O indicate a SiAlON composition. of the chemical system (Si—C—N—O—(H)) which tends to unfavour the atomic rearrangements at the solid state. Indeed, the previous formation and segregation of tetrahedra with appropriate compositions (like SiC4) is necessary to subsequently allow the various phases (like SiC) to crystallise.
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_93.html (1 of 2) [20/01/2010 10:04:04 AM]
page_93
< previous page
page_93
next page >
file:///C|/Users/steppenwolf/Documents/educatio...oks/to%20burn/nanocomposites/files/page_93.html (2 of 2) [20/01/2010 10:04:04 AM]
page_94
< previous page
page_94
next page >
Page 94 The C/N atomic ratio of the as-prepared materials appears to be the leading parameter to determine whether SiC and/or Si3N4 will finally crystallise at some point of the annealing treatment. Starting from a nearly similar Si content, a high C/N content favours the early formation of a SiC phase within a surrounding amorphous matrix, in which heteroatoms (O, N) are subsequently concentrated as an amorphous Si (carbo) oxinitride phase. On the contrary, a low C/N content helps in maintaining the amorphous structure of the bulk at a higher annealing temperature, lately inducing a dramatic nucleation-then-growth of both SiC and Si3N4 phases (Si3N4 only for the lowest C/N ratios). Because nucleation occurs at higher temperatures (>1500°C) with low or no temperature gradient, growth mechanisms (and kinetics) are different, possibly due to a higher mobility of atoms allowing crystals to grow freely, therefore, giving rise to primary crystal morphologies instead of the round, isometric morphology (like that resulting from the flash-temperature nucleation-then-growth mechanism occurring for the gaseous-precursor-based nanopowders). Whatever, polyaromatic C is always the first phase to crystallise, though with a low-dimensionality – turbostratic – structure, according to a common behaviour of Si-based polymer-derived ceramics (Monthioux and Delverdier 1996). Consequently, the amount of it is directly related to the C content of the as-prepared material. SI/C/N/AL-BASED MATERIALS Whether NH3 is present or not in the gas phase, all the as-prepared materials investigated are nearly all amorphous but tend to a two-morphology differentiation with small, nanoporous grains, and larger, nonporous grains, which could be related to the subsequent SiC/Si3N4 phase differentiation. Effect of the 1600°C annealing • Average grain sizes decrease, revealing a weight loss subsequent to the ceramisation process. The crystallised phases mainly depend on the N content of the chemical system. • Not mentioning the polyaromatic C phase, which is not systematic, the SiC phase crystallises prior to the Si3N4/SiAlON phase. • SiC crystals are always coated with an amorphous (Si?)—Al—O phase which is an interesting feature for subsequent attempts of high-temperature sintering. • Correspondingly to the high annealing temperature, the SiC structure is always a mixture of various polytypes (though with various proportions from a material to the other), present as stacking faults rather than as single crystals. Effect of the presence of NH3in the precursor gas phase • After annealing, N-depleted chemical system, induced by the absence of NH3 in the precursor gas phase, on one hand allows the occurrence of a polyaromatic C phase and on the other hand allows the formation of a crystallised SiC phase only (i.e. no Si3N4). • Adding NH3 in the precursor gas phase induces the early crystallisation of SiC. However, the nucleation step does not occur as a widespread germination but occurs locally. Such a heterogeneous behaviour has to be related to a heterogeneity in chemical composition, possibly originating in the non-homogeneous incorporation of N and/or H into the material. On the contrary, the absence of NH3 provides a quite amorphous material.
< previous page
page_94
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_94.html [20/01/2010 10:04:04 AM]
page_95
< previous page
page_95
next page >
Page 95 • Adding NH3 in the precursor gas phase allows the required stoichiometry to be reached, resulting in the rapid crystallisation of a SiAlON-type phase after annealing. Meanwhile, the high temperature at which the overall SiC crystallisation occurs induce such an atom mobility than the respective intrinsic growth rates of the various crystal faces are respected. Effect of varying the NH3concentration in the precursor gas phase • For the lowest and the highest supply in NH3, the prevalent polytype of the resulting crystallised SiC phase after annealing is 3C, corresponding to the β-cubic structure. An intermediate NH3 supply results in a more rapid growth of the SiC phase, for which the other polytypes are correspondingly prevalent. Such a nonmonotonous effect of the increasing N content of the chemical system regarding the behaviour of the material during annealing was already observed for Si-based polymer-derived ceramics and originates from the competition between antagonist mechanisms (Delverdier et al. 1992a). • Increasing the N proportion slows down the kinetics of structural rearrangement; inducing the highest amount of remnant amorphous phases in the N-richest system after annealing. Another reason is also the early crystallisation of SiC prior to Si3N4, which induces a local excess of N atoms relative to the Si atoms left with respect to the required Si3N4 stoichiometry, which then gather into an amorphous phase. • The crystallisation of a nitride phase occurs for a 20% and 40% input of NH3 in the precursor gas phase. In both materials, the high annealing temperature tends to induce the overall crystallisation of massive SiAlON-type crystals rather than Si3N4. In addition, seldom SiAlON needle-like crystals are found in the latter sample (40% NH3), while numerous Si3N4 needle-like crystals are found in the former (20% NH3). Assuming that the massive and needle-like morphologies correspond to α and β structures respectively, these data suggest that the structure change might be somehow controlled by the N content of the chemical system, independently from the extent of Al—Si and O—N substitution. 4.2 As-prepared sintered composites Some of the as-prepared, sintered, micro–nano-type composites, whose detailed processing conditions and mechanical properties are described in Chapter 7, were investigated by TEM to investigate further the structural and textural relationships between the composite components. Related sample preparation prior to TEM investigations and TEM operating conditions are reported in Section 4.3. Sintering temperature was 1650°C for all the composites (1600°C for the bulk Si3N4 material). All the materials (i.e. bulk Si3N4 and composites) are added with the regular sintering aids, Al2O3 and Y2O3, added in the proportions of 3% and 6%, respectively. For technical reasons, all the materials but the bulk Si3N4 were sectioned, thinned and observed in a direction parallel to the hot pressing direction. In the following, after describing the monolithic Si3N4 material, composites will be presented according to the decreasing amount of theoretical SiC content (Table 7.1). 4.2.1 Bulk Si3N4 Monolithic sintered Si3N4 – that is, not added with any nanopowder – was studied as a reference material. The sintering temperature at 1600°C provides the highest densification rate
< previous page
page_95
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_95.html [20/01/2010 10:04:05 AM]
page_96
< previous page
page_96
next page >
Page 96
Figure 4.57 TEM bright-field image from the SiAlON monolithic material. (see Figure 7.6(b)). The sample was investigated in a plane perpendicular to the hot-pressing direction. This plane also contains the direction of mechanical testing. The material appears highly densified (Figure 4.57). Due to the high sintering temperature and the presence of oxides, a dramatic chemical and structural transformation has occurred, inducing a high β-SiAlON (Si6 −zAlzOzN8−z) crystal content (see Section 7.2), about 70% according to calculations based on XRD data (Rossignol 1995), as compared to 100% of α structure in the starting powder (see Section 7.4.1). Correspondingly, a majority of the grains are more or less elongated, some exhibiting an obvious needle-like morphology. This is consistent with previous TEM observations which demonstrated that oriented pressure sintering is able to statistically induce a preferred orientation perpendicular to the pressing direction as far as non-isometric crystals – like high-temperature β-SiAlON or β-Si3N4 – are concerned (Champion et al. 1992). Of course, aspect ratios revealed by TEM are just apparent, since depending on the crystal orientation relative to the sectioning direction for the non-isometric grains. Actually, many of the nearly isometric crystal morphologies are likely to also derive from β-type crystals, that is, about 250–300 nm, while the maximal value observed for the elongated crystal dimension is about 2 μm. Crystals most often exhibit a uniform grey contrast, indicating that they are mainly free of stacking faults. 4.2.2 Si3N4/SiC173 composites The composites investigated were initially prepared with 20% and 40% of SiC173 nanopowder, respectively (Table 7.1). Considering that the starting SiC173 nanopowder is made of quasi pure SiC (with some content of polyaromatic C, see section on Si/C-based powders), such proportions also correspond to the theoretical proportions of the SiC phase in the final composites (Table 7.1).
< previous page
page_96
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_96.html [20/01/2010 10:04:06 AM]
page_97
< previous page
page_97
next page >
Page 97 No obvious discrepancy was found between composite Si3N4/SiC(20) and composite Si3N4/SiC(40) as observed in TEM. The following comments are therefore valid for both materials. Low magnification TEM images are consistent with the theoretical SiC phase proportions (Figure 4.58), and emphasise the size difference between the SiAlON and SiC phases. SiAlON crystals appear as large, polyhedral grains, quite similar to that of the monolithic material (Section 4.2.1). Although diffraction patterns indicate a majority of β structure consistent with the high-temperature sintering (Figure 4.59(a)), a reflection specific of the α phase (at 0.432 nm) is still found sometimes (Figure 4.59(b)), indicating that the structural α to β transformation rate is not 100%, which is consistent with the theoretical calculations (Table 7.3). However, considering that XRD was not able to reveal any α structure, the actual amount of α crystals is surely less than the 11% predicted from calculations (and probably less than 7%, the lowest percentage determined by X-ray in composite Si3N4/SiCN35(22.2)). Most of the crystal facets appear as straight lines, as for single crystals when allowed to grow freely (Figure 4.58). However, crystal facets of SiAlON crystals at the contact of SiC grains often appear notched (see Figure 4.66 for reference) due to the presence of SiC grains at the interface, confirming that SiC grains were not allowed to melt or soften during the sintering process, unlike the growing SiAlON crystals. It is worth noting that only few elongated crystals are found. Calculating an average apparent crystal size is therefore possible: ~470 nm
Figure 4.58 TEM bright-field image from composite Si3N4/SiC(20). The SiC crystals (small, round grains) are gathered into aggregates.
< previous page
page_97
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_97.html [20/01/2010 10:04:07 AM]
page_98
< previous page
page_98
next page >
Page 98
Figure 4.59 Electron diffraction from composite Si3N4/SiC(20). (a) Most of the diffraction spots are characteristic from the β-SiAlON phase. (b) However, some specific diffraction spots (arrow) reveal the minor occurrence of the α structure as well. for composite Si3N4/SiC(40). The slightly lower value for Si3N4/SiC(20) is not significant. Comparison with the monolithic Si3N4 material regarding the evolution of the grain size is limited since it was not investigated along the same section plane. SiC crystals appear as small, round crystals, most often gathered into agglomerates instead of being randomly dispersed all around the SiAlON crystals (Figures 4.58). Contrarily to the latter, SiC crystals exhibit numerous, non-periodical, dark contrasts revealing the occurrence of polytypes as stacking faults. Indeed, the β to α (i.e. polytypes other than β) SiC transformation has slightly progressed, as ascertained by the more frequent occurrence of specific features in the diffraction patterns, like the occurrence of diffraction spots aside the regular diffraction rings for the β structure, and of some aligned spots corresponding to the presence of stacking faults (Figure 4.60 to be compared with Figure 4.3). On the contrary, the average SiC grain size has not progressed significantly compared to the starting powder (see section on Si/C-based powders). This indicates that the growth mechanism by coalescence, though an usual process at such temperatures (Monthioux and Delverdier 1996), was prevented, probably because of the presence of the intergranular phase (Figure 4.62), as opposed to the starting nanopowder (see Section 4.1.1). Some SiC grains are also found possibly enclosed into SiAlON crystals (Figure 4.61). However, high magnification images are not sufficient to ascertain if the SiC crystals are actually enclosed into the SiAlON crystals or if they merely are superimposed to them in the projected image as allowed by the thickness value of the TEM preparation (~100 nm). Proofs of enclosing of SiC crystals into SiAlON crystals will be brought using darkfield imaging (see Figure 4.66 to come). The polyaromatic C phase associated with SiC grains revealed in the starting powder is no longer found, suggesting that it might have burnt into CO during the sintering process. An amorphous, intergranular phase is found, gathering the whole yttrium content of the composite (in addition to some content in the other elements present, Si, Al, O, N) as revealed
< previous page
page_98
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_98.html [20/01/2010 10:04:07 AM]
page_99
< previous page
page_99
next page >
Page 99
Figure 4.60 Electron diffraction from a SiC grain agglomerate in composite Si3N4/SiC(40). Though reflections from the β structure are still prevalent, many other polytypes are present.
Figure 4.61 High magnification TEM image from composite Si3N4/SiC(20). A SiC grain (faulted) seems to be enclosed in the SiAlON crystal. by the darkness of the grey contrast associated to this phase, originating from the intense electron inelastic scattering induced by the high Z value for yttrium (Z = 39). However, most of the intergranular phase is found within SiC grain agglomerates either filling the voids between grains (Figure 4.62) or at the grain interfaces (Figure 4.62, arrows). On the contrary, the intergranular phase is absent between SiAlON crystals (Figure 4.63) or might eventually
< previous page
page_99
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_99.html [20/01/2010 10:04:08 AM]
page_100
< previous page
page_100
next page >
Page 100
Figure 4.62 High magnification TEM image from composite Si3N4/SiC(20). Spaces between SiC grains or at the SiC/SiAlON interface appear dark due to the presence of the yttrium-containing amorphous intergranular phase. be present as some very thin – <1 nm – films only, therefore not visible on lattice fringe images due to the slight tilt angle of the interface relative to the electron beam. It is assumed that such a preferred location of the intergranular phase is due to the faceted morphologies for the SiAlON crystals, whose face-to-face contacts of the respective crystal facets during the hot pressing is likely to expel and reject the intergranular phase into intergranular voids between SiC crystals (Figure 4.62). The latter are numerous in SiC crystal agglomerates due to the round morphology of the grains. 4.2.3 Si3N4/SiCN35 composites The following two composites were prepared with 44.4% and 11.1% of SiCN35 nanopowder, providing a theoretical SiC content of 20% and 5%, respectively (Table 7.1).
< previous page
page_100
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_100.html [20/01/2010 10:04:09 AM]
page_101
< previous page
page_101
next page >
Page 101
Figure 4.63 TEM lattice fringe image from composite Si3N4/SiC(20). The interface between SiAlON crystals is free of interfacial phase. Si3N4/SiCN35(44.4) composite Many of the morphological, textural and structural features described above for the Si3N4/SiC173 composites are valid for this composite. One discrepancy, however, concerns the SiC phase, which now exhibits two kinds of morphology. In addition to the regular, round, major morphology previously described (with about the same grain size range, though slightly lower, 10–60 nm), polyhedral crystals whose sizes range from ~50 to ~150 nm are found as a minor phase (Figure 4.64). Correspondingly to this larger average size, the β to α transformation is more pronounced for this second morphology (see Figure 4.40 for reference, to be compared with Figure 4.60 for the major SiC phase morphology, and with Figure 4.24 for the structural state of the SiC phase in the as-prepared SiCN35 nanopowder). This morphological differentiation indicates at least two distinct sources for the SiC phase, one originating from the pre-existing SiC crystals, the other possibly originating from the crystallisation of the pre-existing Si—C—O—N amorphous phase and/or the reaction of the pre-existing Si phase with any dispersed C atoms. Another discrepancy concerns the SiAlON phase, whose average apparent crystal size is ~360 nm, that is, smaller than for composite Si3N4/SiC173(40). Si3N4/SiCN35(11.1) composite A major difference with the three composites described so far is brought by the SiC phase, which is now more often located between the SiAlON crystals, that is, clearly located in intergranular position (Figure 4.65). Beside, in this sample as in all the other SiC-containing composites described in this chapter, SiC crystals structurally enclosed into SiAlON crystals are found, as clearly demonstrated by the example of the bright-field/dark-field comparison of Figures 4.66(a) and (b). Two SiC crystals supposedly enclosed into a SiAlON crystal are
< previous page
page_101
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_101.html [20/01/2010 10:04:10 AM]
page_102
< previous page
page_102
next page >
Page 102
Figure 4.64 TEM dark-field image (DF2 position) from composite Si3N4/SiCN35(44.4). Example of the minor SiC morphology, exhibiting larger sizes and polyhedral contours, found in addition to the major, regular, round morphology. arrowed in the bright-field image of Figure 4.66(a), to be compared with the specific dark-field image of Figure 4.66(b), whose objective aperture position is adequately chosen so that none of the possible diffracted beams from crystallised SiC are allowed to participate in the image, while the diffracted beam from the SiAlON crystal selected is allowed (see Section 4.3). On Figure 4.66(b), the SiAlON crystal appears dark at the very place of one of the SiC crystal (solid arrow on Figure 4.66(a)), while it appears bright at the very place of the other SiC crystal (open arrow on Figure 4.66(a)) making the latter invisible. The former SiC crystal (solid arrow) is therefore really enclosed into the SiAlON crystal, while the latter SiC crystal (open arrow) is merely superimposed to it in the thickness of the TEM preparation. Contacts between enclosed SiC and surrounding SiAlON crystals were always found direct, that is, with no interfacial phase. Though enclosing of SiC crystals into SiAlON crystals is thus ascertained and supported by the literature (Niihara et al. 1990; Sasaki et al. 1993), examples are actually few in our materials, making doubtful that such nanometric SiC crystals are able to play a substantial role in the germination or phase transformation of the SiAlON crystals in the composites investigated. Meanwhile, Figure 4.66(b) also illustrates how the development of the crystal faces is hindered by the presence of SiC grains in interfacial position, inducing a highly indented topology of the related crystal facets. Decreasing the SiC content in the Si3N4/SiCN35 composites help the SiAlON crystals to develop further, since the average apparent SiAlON crystal size is ~395 nm (as opposed to ~360 nm in composite Si3N4/SiCN35 (44.4)).
< previous page
page_102
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_102.html [20/01/2010 10:04:11 AM]
page_103
< previous page
page_103
next page >
Page 103
Figure 4.65 TEM bright-field image from composite Si3N4/SiCN35(11.1). Light grey contrast-free areas are SiAlON crystals. SiC grains are in interfacial position between SiAlON crystals.
Figure 4.66 Composite Si3N4/SiCN35(11.1). (a) TEM bright-field image. SiC grains are gathered into aggregates. Arrows show examples of SiC grains possibly enclosed in a SiAlON crystal. (b) TEM dark-field image. Imaging conditions (DF1) are adequately chosen to image SiAlON crystals (bright area), while SiC is excluded. One of the SiC grain (solid arrow) is still visible and is therefore really enclosed into the SiAlON crystal, while two other SiC grains (open arrows) have vanished and are therefore merely superimposed to the SiAlON crystal in the projected image. Note how the SiAlON crystal facets are notched due to the contact with SiC grains which have hindered the normal growth. The amorphous intergranular phase is revealed between SiC grains as a slightly scattering phase.
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_103.html (1 of 2) [20/01/2010 10:04:12 AM]
page_103
< previous page
page_103
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_103.html (2 of 2) [20/01/2010 10:04:12 AM]
page_104
< previous page
page_104
next page >
Page 104
Figure 4.67 TEM bright-field image from composite Si3N4/SiCN29(20). Many elongated crystals are found. 4.2.4 Si3N4/SiCN29(20) composite This composite was prepared with 20% of SiCN29 nanopowder, providing a theoretical SiC phase content of 1.7% only. The textural description of the composite is basically similar to that of composite Si3N4/SiCN35 (11.1) described above. SiC grains are again often disseminated in intergranular position between SiAlON crystals. However, SiC crystals are found to exhibit a single morphology, which is consistent with the fact that the SiC source is unique, since no pre-existing SiC nor Si phases were present in the starting nanopowder (see Section 4.1.2). Also, SiC crystals are less numerous, consistently with the calculation, allowing SiAlON crystals to grow and develop more freely than in other composites. Correspondingly, SiAlON crystals very frequently exhibit elongated sections, as opposed to the other composites (Figure 4.67), making an average apparent crystal size difficult to calculate. Grain section range is wide, up to several micrometers for maximal lengths, and 200–400 nm for maximal widths. Although the direct comparison is not allowed with the monolithic Si3N4 material due to the fact that TEM preparations were not performed following the same direction (i.e. perpendicular and parallel to the hot-pressing direction for the monolithic and the composite materials, respectively), the overall impression is that the average crystal size is smaller for the composite (Figure 4.67) than for the monolithic material (Figure 4.57), which is consistent with results from SEM investigations (see Figures 7.8(b) and 7.10, respectively for comparison). 4.2.5 Conclusion regarding as-prepared sintered materials An overall statement is the elimination of the pre-existing polyaromatic C phase – if any – during the sintering process, due the carbo-thermal reduction reaction with the oxide phases added (or pre-existing). This is likely to induce some gas release (CO) possibly responsible for some of the remaining porosity.
< previous page
page_104
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_104.html [20/01/2010 10:04:12 AM]
page_105
< previous page
page_105
next page >
Page 105 Pre-existing SiC grains are stable in the material being sintered, more or less preventing the SiAlON crystals to develop freely. Specifically, SiAlON crystal facets appear flat at the SiAlON/SiAlON contacts, while they appear notched at the SiAlON/SiC contact. When in high proportions (>5% according to the theoretical calculations), the SiC phase tends to gather into agglomerates apart of the SiAlON phase, instead of being dispersed in intergranular position. Agglomeration could be caused by the occurrence of the surrounding minor phase (polyaromatic C in case of SiC173 nanopowder, and an amorphous silicon oxycarbide phase in case of SiCN35 nanopowder), preventing a convenient dispersion during the mixing step prior to making the green bodies (see Chapter 7). Such agglomerates, because they are made of small, round grains having limited surfaces of contact, exhibit a high intergranular porosity allowing to somehow trap most of the yttrium-containing amorphous phase, which is then no longer available to form interfacial films between SiAlON crystal facets. A poor superplastic behaviour is therefore expected for these composites. On the contrary, a low content in SiC nanograins is favourable to a better dispersion in intergranular position between SiAlON crystals. However, SiAlON crystal faces are then prevented to grow freely, the hindering presence of the SiC grains at the SiAlON crystal interfaces while developing from the liquid phase inducing indentations in the related crystal faces. SiC grains thus act as ‘keystones’ between SiAlON grains, which is also detrimental to a superplastic behaviour. Nano/nano composites are therefore expected to be preferable to micro/nano composites regarding the ability to creep without developing cracks. Further and extended comments will be found in Chapter 7. 4.3 TEM sample preparation prior to investigations and operating conditions 4.3.1 Preparation of samples In order to be electron transparent at 120 kV acceleration voltage, materials investigated should exhibit a thickness ideally lower than 100 nm in the direction parallel to the electron beam. Ceramic nanopowders therefore require limited efforts for TEM preparation, considering the convenient initial grain sizes. On the contrary, composites require a specific thinning process. Powders Aliquots of each ceramic nanopowder were dispersed into ethanol under sonication for several minutes in order to make a suspension from which a drop was then deposited on a regular (3 mm) 200 mesh copper microgrid previously coated with a holey or a lacey amorphous C film. For samples suspected to be possibly hydrolysable, dry preparation – that is, direct deposition of the nanopowder onto the microgrid – were sometimes also made for double checking. When large powder agglomerates were formed unable to be dismantled by the wet sonication step, gentle grinding using a boron carbide mortar was previously made (use of a silica mortar should be avoided, due to its lower hardness relative to SiC, which is likely to provoke some input of silica into the sample being prepared). The main limitation of such a preparation procedure is the possibility to induce a gravimetric discrimination – the phases exhibiting much higher density, or much larger grains being likely to sink to the bottom of the flask.
< previous page
page_105
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_105.html [20/01/2010 10:04:13 AM]
page_106
< previous page
page_106
next page >
Page 106 Sintered materials A slice about 100 μm thick of each sintered materials was obtained using a diamond-coated slow circular-saw (preferably to a diamond-coated tungsten-wire saw, whose efficiency was limited in this specific case). The slice dimensions was then adjusted to fit in a 3-mm wide copper aperture, then glued on a stainless steel support using a thermofusible resin. Then the thickness of the slice was decreased down to ~50 μm using a mechanical polishing procedure involving submicrometric diamond powders. The slice was then reversed upside down in order to complete the polishing/thinning process through the other side of the slice, hopefully down to ~20 μm. The slice was then glued onto a 3-mm copper aperture, then ion-milled both sides for several hours. Acceleration voltage for the argon ions was ~4kV, and ion gun direction angles with respect to the sample surface were 12–15°. A hole was created, whose edges were suitable for the TEM investigation. All the micro/nano composites investigated (specifically those with a high SiC content) were more or less found to specifically exhibit a very high hardness making them unusually difficult to slice during the first step of the procedure (diamond-enhanced sawing), as opposed to the behaviour of regular micro/micro-type composites (such as in Champion et al. 1992). On the contrary, the micro/nano composites were found to dismantle more easily than regular micro/micro composites at the end of the polishing/thinning procedure. A possible explanation is that the primary specifically high hardness is due to the lack of amorphous intergranular phase at the SiAlON crystal interfaces, making the crystals collectively supporting the shearing stresses developed during the sawing procedure as a monolithic single crystal would do. On the other hand, the removal of SiC grain agglomerates is easier during the next polishing/thinning step due to their high content in amorphous phase. This is likely to promote the earlier dismantling of the composite with respect to micro/micro composites, as soon as a critical limit (~50 μm) for the slice thickness is reached. 4.3.2 TEM operating procedure We do not intend to describe all about the principle of electron imaging. The goal of this section is merely to provide to the non-microscopist reader the keys needed to understand the comments reported in this chapter. Basics and more about the principles of TEM can be found in Williams and Carter (1996). About dark-field mode imaging Contrasted bright field and lattice fringe are two regular imaging modes involving the use of apertures with suitable opening diameters placed in the back focal plane of the objective lens. For the non-microscopist reader, considering the electron microscope as a powerful, high-resolution magnifying lens able to image down to the lattice planes of crystals is enough to understand the kind of comments made in this chapter. Likewise for the selected area electron diffraction, whose principles are similar to that of XRD. However, further explanation might be useful to fully understand the data brought by the dark-field imaging mode. Although a TEM may contain seven or more electromagnetic lenses, its main quality and mode abilities depend on the objective lens. As for regular, optical glass lenses, electromagnetic lenses are characterised by three planes: the focalisation plane (where the specimen should be located for its image to be focused on the image plane), the focal plane (specifically the back focal plane, which contains the electron diffraction patterns in the case of the objective lens), and the image plane, where the enlarged image of the specimen is formed
< previous page
page_106
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_106.html [20/01/2010 10:04:13 AM]
page_107
< previous page
page_107
next page >
Page 107
Figure 4.68 Sketch of the electron beam paths in the objective lens of a microscope. (a) Bright-field image, (b) dark-field image.
Figure 4.69 Examples of various positions of the objective aperture relative to the diffraction pattern of a multiphase material (β-SiC + turbostratic C) used to perform specific dark-field imaging. (Figure 4.68(a)). Placing an aperture (so-called objective aperture) in the back focal plane of the objective, therefore, allows specific electron beams to be selected, that is, the image is built with some electron beams only (Figure 4.68(b)). For instance, selecting a specific diffracted beam with the objective aperture results in an image whose bright parts indicate the regions of the specimen from which the selected diffracted beam is emitted, while everywhere else, in or around, the specimen appears dark (or nearly). It is then already quite clear that, by successively selecting adequately various positions for the objective aperture, sequential dark-field images can be formed which can be specific of different orientations for a single crystallised phase, or of different phases within a multiphase material, or both. This principle is illustrated in Figure 4.69, with the example of a material
< previous page
page_107
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_107.html [20/01/2010 10:04:14 AM]
page_108
< previous page
page_108
next page >
Page 108 containing both β-SiC and polyaromatic, turbostratic C. The related theoretical diffraction patterns are both represented. Positioning the aperture in DF1 allows part of the C002 diffracted beams to go through, and to build the image of polyaromatic entities – if any – whose (001) lattice planes are oriented both parallel to the electron beam (i.e. graphenes are seen edge-on) and parallel to the E–W direction (or nearly, since the width of the aperture is such that it admits an arc instead of a single dot). Then, positioning the aperture at 90° along the same diffraction ring (position DF1⊥) will image other polyaromatic entities – if any – oriented S— N, that is, perpendicularly to the former. The related two images are exclusive from SiC crystals and are therefore specific of the C phase. SiC crystals will in turn be able to be imaged by using position DF2. In that case, rotating the aperture relative to the diffraction pattern all along the SiC111 diffraction ring (meanwhile also rotating along the SiC200 ring, which is very close) will successively reveal any SiC crystal oriented so that they present (111) or (100) reticular planes parallel to the electron beam. It is worth noting that the DF2 position is not really specific of a SiC phase, strictly speaking, since the aperture width is such that the 10 diffraction band of turbostratic C is also admitted, allowing the related electrons to participate in building the image (using smaller apertures would be too much detrimental to the resolution). Graphene stack entities oriented perpendicularly to the electron beam (i.e. lying flat on the specimen support grid) are thus supposed to be imaged together with the SiC crystals. Practically, due to the intensity of the SiC111 reflection, by far much higher than for the C10, DF2 images are considered specific of a SiC phase in most cases. Because the objective aperture is placed in various positions relative to the diffraction pattern, such dark-field imaging sequences are said to correspond to a radial and azimuthal exploration of the reciprocal space. For this reason, the objective aperture apparent widths are given in nm−1. TEM operating conditions Bright-field, dark-field, lattice fringe and selected area diffraction mode images were obtained using a Philips EM400 microscope operating at 120 kV and equipped with a high-resolution stage providing a point resolution better than 3 Å, with a tungsten wire as electron source. The width of the aperture used for the contrasted bright-field and lattice fringe imaging was 8nm−1, while that used for dark-field imaging was 2 nm −1. According to the Abbe relation where λ is the wavelength and a the half-width of the aperture (in radians) using an objective aperture as small as 2 nm−1 reduces the resolution ρ to ~6 Å. Dark-field imaging was carried out most often using DF1 (aperture centred at 2.2nm−1) and DF2 (aperture centred at 4.3nm−1) positions described in the previous section. Considering the width of the aperture opening, the radial tolerance regarding the frequency range admitted for both positions are 1.3–3.3nm−1 and 3.3–5.3nm−1, respectively. Likewise, the azimuthal deviations relative to the centring position due to the aperture opening are ±24° and ±15°, respectively. Attention has to be paid that, depending on the phases present in the material investigated, the specificity of the positions may vary. For instance, the powder diffraction pattern for a Si3N4 phase exhibits numerous diffraction rings (Figure 4.20 for instance), making Si3N4 crystals likely to be imaged in any possible position for the objective aperture, including DF1 and DF2. Also, other aperture positions were sometimes used, for specific purposes. Finally, though they do not provide diffracted beams strictly speaking, but are anyway able to scatter electrons in some specific directions because of short-range structural periodicities (often around
< previous page
page_108
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_108.html [20/01/2010 10:04:15 AM]
page_109
< previous page
page_109
next page >
Page 109 the most intense diffracted beam for the related crystallised material), so-called amorphous materials are likely to also appear in dark-field images. For instance, amorphous silica may be revealed in DF1 position, providing an intense halo at 0.44 nm−1 (Chaudhari et al. 1972), while the most intense reflection for any form of crystallised silica is located at ~0.41 nm−1. X-EDS spectroscopy was performed using a Philips CM20 microscope equipped with a high-resolution goniometric stage (super-twin stage) and an EDAX detector (Li-doped silicon diode), protected by an ultrathin window allowing the detection of chemical elements including light elements down to C. References Audier, M., Oberlin, A., Oberlin, M., Coulon, M. and Bonnetain, L. (1981) Carbon, 19, 217. Badami, D. V. (1965) Carbon, 3, 53. Buffat, P. and Borel, J.-P. (1976) Phys. Rev. A, 13, 2287. Champion, E., Goursat, P., Besson, J. L., Madigou, V., Monthioux, M. and Lespade, P. (1992) Ceram. Eng. Sci. Proc., American Ceramic Society, USA, p. 732. Chaudhari, P., Graczyk, J. F. and Herd, R. (1972) Phys. Stat. Sol., 51, 801. Delverdier, O., Monthioux, M., Mocaer, D. and Pailler, R. (1992a) Proc. 5th Eur. Conf. Compos. Mater., (eds A. R. Bunsell, J. F. Jamet and A. Massiah), Bordeaux, France, p. 691. Delverdier, O., Monthioux, M., Oberlin, A., Lavedrine, A., Bahloul, D. and Goursat, P. (1992b) High Temp. Chem. Proc., 1, 139. Delverdier, O., Monthioux, M., Mocaer, D. and Pailler, R. (1993) J. Eur. Ceram. Soc., 12, 27. Delverdier, O., Monthioux, M., Mocaer, D. and Pailler, R. (1994) J. Eur. Ceram. Soc., 14, 313. Iijima, S. (1982) Solid State Chem., 42, 101. Inoue, Z. and Kourachi, Y. (1983) Proc. Int. Symp. Ceram. Components Engines, Japan, p. 519. Laanani, Fadéla (1997) Thèse de Doctorat, no 2707, Université Paul Sabatier, Toulouse, France. Le Coustumer, P., Monthioux, M. and Oberlin, A. (1993) J. Eur. Ceram. Soc., 11, 95. Madigou, Véronique, Monthioux, M. and Oberlin, A. (1990a) Proceedings of Matériaux Composites pour Applications à Hautes Températures (eds R. Naslain et al.), AMAC-CODEMAC, Bordeaux, France, p. 221. Madigou, Véronique, Monthioux, M. and Guimon, C. (1990b) Proc. XX Int. Conf. Carbon, GFEC, Paris, France, p. 220. Madigou, Véronique (1991) Thèse de Doctorat,n°116, Université de Pau et des Pays de l’Adour, France. Mocaer, D., Pailler, R., Naslain, R., Richard, C., Pillot, J.-P., Dunoguès, J., Delverdier, O. and Monthioux, M. (1993) J. Mater. Sci., 28, 2639. Monthioux, M. and Delverdier, O. (1996) J. Eur. Ceram. Soc., 16, 721. Monthioux, M., Oberlin, A. and Bouillon, E. (1990) Compos. Sci. Technol., 37, 21. Niihara, K., Suganuma, K., Nakahira, A. and Izaki, K. (1990) J. Mater. Sci. Lett., 9, 598. Oberlin, A. (1989) Chemistry and Physics of Carbon, vol. 22 (ed. P. A. Thrower), Marcel Dekker, New York, p. 1. Oberlin, A. and Rouchy, J.-P. (1971) Carbon, 9, 39. Oberlin, A., Oberlin, M. and Comte-Trotet, J. R. (1976) J. Microsc. Spectrosc. Electron., 1, 391. Oberlin, A., Boulmier, J. L. and Villey, M. (1980) Kerogen (ed. B. Durand), Technip, Paris, p. 191. Oberlin, A., Bonnamy, S., Bourrat, X., Monthioux, M. and Rouzaud, J.-N. (1986) Petroleum Derived Carbons (eds J. D. Bacha, J. W. Newman and J. L. White), ACS Symposium Series 303, USA, p. 85. Okamura, K., Sato, M., Hasegawa, Y. and Amano, T. (1984) Chem. Lett., 2059. Rossignol (1995) Thèse de Doctorat, Université de Limoges, France. Sasaki, G., Suganuma, K., Fujita, T., Hiraga, K. and Niihara, K. (1993) Mater. Res. Soc. Symp. Proc., 287, 335. Williams, D. B. and Carter, C. B. (1996) Transmission Electron Microscopy. A Textbook for Materials Science, Plenum Press, New York.
< previous page
page_109
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_109.html [20/01/2010 10:04:15 AM]
page_110
< previous page
page_110
next page >
Page 110 5 From short- to long-range order Structural organisation of silicon-based nanopowders
< previous page
page_110
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_110.html [20/01/2010 10:04:15 AM]
page_111
< previous page
page_111
next page >
Page 111 5.1 Chemical order studied by solid-state nuclear magnetic resonance André Pierre Legrand, Jean-Baptiste d’Espinose de la Caillerie and Youssef El Kortobi Native or heat-treated ceramics contain different atoms, the nuclei of which can be used, if provided with a magnetic moment, as NMR probes. Among them 1H,13C,27Al and 29Si are of particular interest. Different information can be obtained, depending on the method of observation and on the nature of the nucleus under analysis. Each proton has a magnetic moment (1H) and is relatively easy to observe. Nevertheless, it physically interacts through dipole–dipole interactions. This induces a line broadening of the spectrum, which can hide the chemical information concerning the different chemical species on, and inside ceramics (hydroxyls, water, etc.). So different approaches are possible by taking advantage of this dipolar interaction or on the contrary by suppressing it. Silicon nucleus (29Si), on the contrary to 1H, is an isotope with a low natural abundance of 4.7%. The same is true for 13C (1.1%). For as-formed ceramics, these diluted species are in dipolar interaction with the abundant proton (1H) species. To observe the nature of the different chemical species in the material, it is necessary to suppress this dipolar interaction. This is obtained through specific techniques. Aluminium nucleus (27Al) has a natural abundance of 100%. Contrarily to the previous nuclei, 27Al is not a Its quantum number is 5/2. This has positive and negative effects. A positive one is that the nucleus spin is sensitive to the local electric field gradient and consequently this gives an important information on the symmetry of the aluminium sites. The negative one is that if the electric field gradient from one site to another site is different, for example, tetrahedral to octahedral, the quantitative determination of the relative proportions could be questionable. 5.1.1 Nuclear magnetic methods As mentioned above, the as-formed amorphous ceramics may contain hydrogen atoms belonging to different chemical species such as hydroxyls and adsorbed water molecules. They constitute a set of 1H spins which, by dipolar interaction, produce a line broadening hiding the chemical information. This harmful effect disappears by heat treatment, with the expulsion of protonated species. 5.1.1.1 Rare spin half spectroscopy (29Si, 13C) Considering the low abundance of 29Si, 13C isotopes, the dipolar interaction responsible for line broadening is mainly due to neighbouring protons, for as-formed ceramics. To determine
< previous page
page_111
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_111.html [20/01/2010 10:04:16 AM]
page_112
< previous page
page_112
next page >
Page 112 the nature of the different functionalities of such nuclei in ceramics, it is necessary to use specific techniques. High power decoupling (HPD) To suppress the unwanted proton-rare spin dipolar interaction, the following method can be used. It requires application of a strong radio frequency field at the Larmor frequency of the abundant spins. Through this operation, the populations of spins in the low and high Zeeman energy levels are made equal and the resulting magnetisation falls to zero, leaving only the chemical shift interaction to be studied (Bloch 1958). Averaging the chemical shift anisotropy (CSA) – Magic angle spinning (MAS) The method involves putting the sample into a rotor, the axis of rotation of which is at an angle of rotation of 54.73° with the external magnetic field. This method is efficient not only to average the dipolar interaction, when MAS speed is high enough, but also the CSA (Engelhardt and Michel 1987). The chemical shift has a theoretical expression that is mathematically similar to that of the dipolar interaction. It is composed of an isotropic value, similar to that observed in liquid state, and an anisotropic part. In consequence, for a powder, this term produces a line broadening, due to the superposition of all possible orientations of the chemical species studied. This requires that the speed of rotation be high enough relatively to the CSA. If not, a more complex spectrum appears which is composed of the mere spectrum, flanked on either side with more or less intense replicas of this one. These satellites are separated by multiples of the rotation frequency. The different isotropic lines are characterised by a position in frequency with respect to a given reference, tetramethylsilane (TMS) in this book, and consequently can be identified. Numerous experiments in solids have demonstrated that the observed chemical shifts are near what is observed in liquids, if the environment is the same. Data already collected for species in solution can therefore be used to analyse solidstate spectra (Lippmaa et al. 1982; Lippmaa and Samoson 1982; Engelhardt and Michel 1987; Fyfe 1983; Marsmann 1981). As the technology has improved, allowing in particular to increase the MAS speed, it is possible to achieve such measurements using higher magnetic fields than previously, which enables increasing resolution and sensitivity. Cross-polarisation (CP) For as-formed ceramics containing an important amount of hydrogen, this method is jointly used with MAS to enhance the signal of carbon (C) or silicon (Si) bonded to protons. First, it involves cooling down the proton reservoir through a sequence shown in Figure 5.1.1. Second is the time to transfer the low temperature of the proton reservoir to that of rare spins. Last is to observe the signal of the rare spin while at the same time using the HPD. The method is consequently denominated CP/MAS. The complete sequence is represented in Figure 5.1.2. Model compound example Role and interest of the different methods mentioned above are summarised in Figure 5.1.3. 29Si NMR spectra of a powdered sample of pure cubic octamer silicic trimethylsilyl ester
< previous page
page_112
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_112.html [20/01/2010 10:04:16 AM]
page_113
< previous page
page_113
next page >
Page 113
Figure 5.1.1 Setting of a spin temperature for the abundant spins (observation in a plane perpendicular to the director field B0): (a) the magnetisation is brought in the perpendicular plane after a 90° pulse; (b) the radio frequency field B1 is phase shifted by a 90° angle, bringing it parallel to the magnetisation; (c) after a certain time, the magnetisation decreases slowly in the B1 field and is measured after switching this field off, on the free induction decay. The upper part of the figure represents schematically the application of radio frequency pulses along the O x and O y axis in the rotating frame. (Reproduced with permission of John Wiley & Sons from Legrand et al. 1998.)
Figure 5.1.2 Complete sequence of CP for abundant spins (e.g. protons 1H) in interaction with less abundant spins (e.g. silicon 29Si). (Reproduced with permission of John Wiley & Sons from Legrand et al. 1998.)
< previous page
page_113
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_113.html [20/01/2010 10:04:17 AM]
page_114
< previous page
page_114
next page >
Page 114
Figure 5.1.3 Rare spin 29Si solid state NMR spectra at 59.6 MHz of a powdered pure cubic octamer silicic trimethylsilyl ester (Q8M8) as model compound, showing the influence of different types of NMR measurements: (a) static or broadband spectrum with no high power decoupling of the protons. Only a broad line is observed: no chemical information is available; (b) static or broadband spectrum with high power decoupling of protons. Two bands, due to chemical anisotropy, corresponding to two Si are observed: no clear chemical identification available; (c) HPD with CP (contact time 1 ms) and MAS with a speed or rotation not high enough (567 Hz). Chemical information partially available; (d) CP/MAS + HPD. Chemical information available. (Courtesy of P. Tougne.) (Q8M8) present the following aspects: 1 With static or broadband method, only broad lines mainly due to the dipolar interaction 1H—29Si are observed. No chemical information is available. 2 As above, with HPD of the protons, CSA of two Si types are observed. 3 CP/MAS method, but with MAS speed of 560 Hz. Side bands with the mere spectrum are observable. 4 CP/MAS method, with MAS speed high enough. Side bands are suppressed and the spectrum shows a triplet and a quadruplet.
< previous page
page_114
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_114.html [20/01/2010 10:04:17 AM]
page_115
< previous page
page_115
next page >
Page 115 5.1.1.2 Aluminium 27Al NMR spectroscopy Unlike 29Si or 13C, 27Al has an I = 5/2 spin and therefore a nuclear quadrupole moment. This implies that not only this nucleus is sensitive to the chemical shift and dipolar interactions but also to the quadrupolar one. The six energy levels (2I + 1) of the 27Al due to the Zeeman effect are modified, assuming a first-order perturbation effect, which results in five different transition frequencies. The corresponding Hamiltonian is:
(5.1) where eQ is the nuclear quadrupolar moment and Vzz = eq, the main electric field gradient (|Vzz| > |Vyy| > | Vxx|); η = (Vyy − Vxx)/Vzz is the asymmetrical parameter. Oxyz are principal axes of the tensor that describe the electric field gradient. All transitions except the central one are subject to a firstorder quadrupolar interaction depending on the orientation of the electric field gradient tensor with respect to the external magnetic field. Since in powder samples there is a random distribution of such orientations, it results in a large spreading of the line which prevents its observation. On the contrary, the central line is only sensitive to the second-order perturbation effect, which causes a line spreading proportional to (e2Qq/h) 2/νL = νQ, where νL is the Larmor frequency of the 27Al nucleus. Contrarily to spin half, the observation is not obtained with a 90° pulse, although this one is obtained with a solution of aluminium salt, in which the Brownian motion averages the quadrupolar effect. Samoson and Lippmaa (1983) proved that the signal intensities are independent of the magnitude of νQ only if the pulse length is short enough. For an error less than 5% in the signal intensity for the centre band of the central transition the spin flip angle ω1τ must satisfy the condition ω1τ(I + 1/2) ≤ π/6, with I = 5/2 for 27Al. |Vzz| > |Vyy| > |Vxx|); η = (Vyy − Vxx)/Vzz is the asymmetrical parameter. Oxyz are principal axes of the tensor that describe the electric field gradient. All transitions except the central one are subject to a first-order quadrupolar interaction depending on the orientation of the electric field gradient tensor with respect to the external magnetic field. Since in powder samples there is a random distribution of such orientations, it results in a large spreading of the line which prevents its observation. On the contrary, the central line is only sensitive to the second-order perturbation effect, which causes a line spreading proportional to (e2Qq/h)2/νL = νQ, where νL is the Larmor frequency of the 27Al nucleus. Contrarily to spin half, the observation is not obtained with a 90° pulse, although this one is obtained with a solution of aluminium salt, in which the Brownian motion averages the quadrupolar effect. Samoson and Lippmaa (1983) proved that the signal intensities are independent of the magnitude of νQ only if the pulse length is short enough. For an error less than 5% in the signal intensity for the centre band of the central transition the spin flip angle ω1τ must satisfy the condition ω1τ(I + 1/2) ≤ π/6, with I = 5/2 for 27Al. An example of the influence of the pulse duration on the relative intensities of the lines is given in Figure 5.1.4 for 23Na (spin 3/2). Such quadrupolar and line shifts render more difficult the interpretation of the line structure but are able to provide additional information of the charge distribution (Figure 5.1.5). 5.1.1.3 Interest of the method The chemical shift of the nuclear resonance provides an incredibly delicate fingerprint of the chemical functionality of an element in a compound. NMR has provided chemists with one of the most powerful qualitative and quantitative analytical tools available to the chemist, material scientist and medical technician. The advent of high-resolution techniques appropriate to nuclei in solids supplied further dimensions to do qualitative analysis of chemical functionalities. Moreover, some information concerning structure and local organisation of clusters can be obtained. Such a method had been largely used for ceramic characterisation (Müller 1999; Templin et al. 1999). 5.1.2 SiC powders analysis In Figure 5.1.6, the 29Si spectrum for sample as-formed SiC163 is shown. Like previously published spectra of silicon carbide powders (Table 5.1.1), it consists of a superposition of two kinds of line: a single line at −16.0 ppm can be attributed to the β-SiC type, whereas the triplet consisting of lines at −15.6, −20.5 and −24.9 ppm can be attributed to α-SiC polytypes.
< previous page
page_115
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_115.html [20/01/2010 10:04:18 AM]
page_116
< previous page
page_116
next page >
Page 116
Figure 5.1.4 2D solid state 23Na MAS–NMR spectra at 79.39 MHz of sodium chlorine and nitrite salts. (a) Influence of the pulse length (from 0.25 to 5 μs, by step of 0.25 μs) on the relative intensities of the two sodium sites; (b) Relative proportion has to be evaluated at short pulse length (here 1:6). (Courtesy of P. Tougne.) As the experimental high-resolution solid-state NMR technique involves only MAS, the spectra can be decomposed and the amount of each type, α-SiC or β-SiC, is proportional to the respective areas of the
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_116.html (1 of 2) [20/01/2010 10:04:19 AM]
page_116
different lines, if the repetition time for accumulation is long enough relatively to the spin-lattice relaxation times. The 29Si spectrum of SiC174 is very similar to the previous spectrum except that the amount of α-SiC has decreased a little.
< previous page
page_116
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_116.html (2 of 2) [20/01/2010 10:04:19 AM]
page_117
< previous page
page_117
next page >
Page 117
Figure 5.1.5 Solid state 27Al MAS–NMR spectrum at 130.32 MHz of gibbsite and saponite. MAS speed: 12 kHz. Clear distinction between four- and sixfold coordinated aluminium in AlO4 and AlO6 units is observed. 27Al chemical shifts are between +50 and +80 ppm for AlO4 and about −10 to +20 ppm for AlO6.
Figure 5.1.6 Solid state 29Si MAS–NMR spectra at 59.6 MHz of as-formed silicon carbide (duty cycle, 500 s; 90° pulse, 5 μs; number of scans, 161, 100, 164 and 60). Spectra are classified as function of decreasing residence time into the laser irradiation cell (Table 2.1). (Reprinted from Tougne et al. (1993) Diamond Relat. Mater., Evolution of the structure of ultrafine SiC-laser-formed powders with synthesis conditions, 2, 486– 490, with permission from Elsevier Science.)
< previous page
page_117
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_117.html [20/01/2010 10:04:19 AM]
page_118
< previous page
page_118
next page >
Page 118 Table 5.1.1 29Si chemical shift in ppm/TMS for silicon carbides Authors Polytype 3C (C) 6H (A B C) 15R (A B C) 4H (B C) 2H (D) Finlay et al. 1985 −18.3 −13.9 −20.2 −24.2 Guth et al. 1987 −18.4 −16.1 −14.3 −20.4 −24.9 −14.6 −20.5 −24.1 Hartman et al. 1987 −18.3 −13.9 −2.02 −24.5 −14.9 −20.8 −24.4 Wagner et al. 1989 −18.4 −16.1a Dando and Tadayyoui 1990 −16 −14.4 −20.5 −25 −15.2 −20.2 −24 Apperley et al. 1991 −18.4 −14.7 −20.9 −25.4 −19.7 −22.5 −20 Schmidt et al. 1991–2 −18 −14 −20 −25 Richarson et al. 1992 −14.5 −20.4 −25.1 Dybowski et al. 1996 −16 −22 −27 Tateyama et al. 1997 −18.4 −14.7 −19.7 −25.4 −20.9 −22.5 −20 Note a Depends on the crystalline structure of the sample (−16.1 for small single crystals). No quantitative accurate decomposition has been performed but it is qualitatively apparent from the spectra. Moreover, on comparing the figure which shows the spectrum for sample as-formed SiC173 with the figure which shows the spectrum for sample SiC177 the trend follows the same line. Increasing the residence time into the hot region of the cell where the synthesis takes place results in a decreasing amount of α-SiC phase. To assess this evolution, samples as-formed SiC163 and SiC177 were annealed in a furnace at 1600°C for 24 h. Figure 5.1.7 shows the spectra of the annealed samples SiC163 and SiC177. One single line at −16.0 ppm now appears which can unambiguously be attributed to a pure β-SiC phase, it appears therefore rather surprisingly that the β-SiC phase is the high temperature stable phase. By comparing the evolution of samples SiC163 and SiC171, one can study the effect of heat treatment. Table 5.1.2 shows that the grain growth occurs at a higher temperature for sample SiC171 than for sample SiC163. At 2000°C, the densification of sample SiC171 is 94% but the grain size has become comparable to the grain size of a commercial powder. The problem is then to achieve good densification and conserving a fine structure. A good knowledge of the local structure evolution would be very helpful. Figure 5.1.8 presents the NMR spectra of samples SiC163 and SiC171 after heat treatment between 1600°C and 2050°C. One can see that the α-phase is always present in sample SiC171, while it almost disappears in sample SiC163 between 1700°C and 1900°C. At 2050°C, β-phase is transformed into α polytypes. 6H, 15R and 4H polytypes are unambiguously identified in sample SiC171 while only the 6 H environment is in sample SiC163. It seems then that there is a relation between the annealing and the presence of the α-SiC polytypes.
< previous page
page_118
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_118.html [20/01/2010 10:04:20 AM]
page_119
< previous page
page_119
next page >
Page 119
Figure 5.1.7 Solid state 29Si MAS–NMR spectra at 59.6 MHz of 1600°C (24 h) annealed silicon carbide (duty cycle, 500 s; 90 ° pulse, 5 μs; number of scans, 69 and 57). (Reprinted from Tougne et al. (1993) Diamond Relat. Mater., Evolution of the structure of ultrafine SiC-laser-formed powders with synthesis conditions, 2, 486–490, with permission from Elsevier Science.) Table 5.1.2 Surface of different silicon carbide batches as a function of temperature dwell (dwell duration: 1 h) Temperature (°C) SBET (m2/g) SiC171 SiC163 SiC177 1600 24.9 13.2 8.1 1800 3.7 7.3 3.3 2000 0.09 5.3 2.3 5.1.3 Si/C/N powders analysis 5.1.3.1 29Si and 13C solid-state MAS–NMR measurements Well-crystallised silicon nitrides have been analysed and 29Si chemical shifts of the two main α and β structures had been determined (Table 5.1.3). Average chemical shift identification of different Si environments in Si/C/N compounds has been done by comparison between pure silanes and pure silicon carbide or silicon nitride. Analysis of the results is given in Table 5.1.4. Besides, different authors have estimated the presence in less organised compounds of Si environments as SiCN3, SiC2N2 and SiC3N (Seitz et al. 1996; Gérardin et al. 1997; Verdecia
< previous page
page_119
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_119.html [20/01/2010 10:04:20 AM]
page_120
< previous page
page_120
next page >
Page 120
Figure 5.1.8 Evolution of 29Si MAS–NMR spectra of sample 163 and 171 as a function of the temperature (dwell duration 1 h). Top of β-SiC peak had been cut to observe polytypes signal. Table 5.1.3 Chemical shift of 29Si in ppm/TMS for crystallised amorphous silicon nitrides. Values within parentheses are full-width at half-height of each peak Authors β-Si3N4 (singlet) α-Si3N4 (doublet) equal intensities Amorphous Carduner et al. 1987, 1990 −48.7 (2.5) −46.8 (1.8) −48.9 (1.8) −46.4 (27) Harris et al. 1990 −48.5 (1.3) −47.1 −49 Table 5.1.4 29Si average chemical shift of different silicon nitrides. Chemical shift measurements done on silane series (upper part) exhibit an average shift of −20 ppm comparatively to pure silicon carbide and silicon nitride. Consequently interpolation is done for intermediary environment of the Si (lower part) Silane Chemical shift (ppm/TMS) (CH3)4Si 0 (CH3)3SiN(CH3)2 6.9 to 5.0 (CH3)2Si(N(CH3)2)2 −1.3 to 1.85 (CH3)Si(N(CH3)2)3 −16.3to−17.5 Si(N(CH3)2)4 −28.1to−28.6 Silicon environment in solid state Average chemical shift (ppm/TMS) SiC4 −20 SiC3N −13 to −14 SiC2N2 −21 to −22 SiCN3 −36 to −37 SiN4 −46 to −49
< previous page
page_120
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_120.html [20/01/2010 10:04:21 AM]
page_121
< previous page
page_121
next page >
Page 121
Figure 5.1.9 Chemical shift of 29Si in ppm/TMS for crystallised SiCxN4−x compounds as a function of the HTT of different ceramics from Seitz et al. (1996), Gérardin et al. (1997) and Verdecia et al. (1998). Symbols are ■ SiN4, ● SiCN3 and ◆ SiC2N2; highest temperature is for well-crystallised silicon nitrides (Carduner et al. 1987, 1990). et al. 1998). Chemical shifts of such Si environments are dependent on the first and second sphere of coordinence. This one is able to contain hydrogen atoms for as-formed or low heat-treated materials and consequently the chemical shift is susceptible to modifications. Figure 5.1.9 summarises different observations. Series HMDS41 to HMDS44, heat-treated from 1000°C to 1600°C in N atmosphere during 1 h, have been analysed using 29Si MAS–NMR. This method enables us to distinguish, through previous mentioned observations given in Figure 5.1.9, the evolution of the local structure around Si. Figures 5.1.10 and 5.1.11 give the general results of the survey. They are classified as a function of the initial C/Nini composition or of the heat-treatment temperature (HTT). Some remarks have to be made: • At HTT 1000°C, no important differences are observable. A broad massif centred around −50 ppm demonstrates an amorphous silicon nitride environment. Besides, a shoulder near −35 ppm can be attributed to SiCN3, the importance of which decreases with initial C/N ratio. A small peak at −110 ppm corresponds to silica.
< previous page
page_121
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_121.html [20/01/2010 10:04:21 AM]
page_122
< previous page
page_122
next page >
Page 122
Figure 5.1.10 Solid state 29Si MAS–NMR spectra at 99.36 MHz, rotation frequency of 5 kHz, of HMDS file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_122.html (1 of 2) [20/01/2010 10:04:22 AM]
page_122
powders heat-treated during 1 h in N atmosphere, as a function of the initial C/N (atomic number) composition, at increasing temperature. (a) HMDS41 (duty cycle, 500 s; 90° pulse, 5 μs; number of scans, 160, 160, 160, 12, 84); (C/N)ini = 0.95; (b) HMDS42 (duty cycle, 500 s; 90° pulse, 5 μs; number of scans, 160, 103, 160, 75); (C/N)ini = 0.73; (c) HMDS43 (duty cycle, 500 s; 90° pulse, 5 μs; number of scans, 144, 125, 140, 120, 81); (C/N)ini = 0.67; (d) HMDS44 (duty cycle, 500 s; 90° pulse, 5 μs; number of scans, 150, 160, 102, 40); (C/N)ini = 0.57.
< previous page
page_122
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_122.html (2 of 2) [20/01/2010 10:04:22 AM]
page_123
< previous page
page_123
next page >
Page 123
Figure 5.1.11 Solid state 29Si MAS–NMR spectra of HMDS powders. Experimental conditions are given in file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_123.html (1 of 2) [20/01/2010 10:04:23 AM]
page_123
Figure 5.1.10 caption. (a) 1000°C/N2/1 h; (b) 1400°C/N2/1h; (c) 1500°C/N2/1 h; (d) 1600°C/N2/1h.
< previous page
page_123
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_123.html (2 of 2) [20/01/2010 10:04:23 AM]
page_124
< previous page
page_124
next page >
Page 124 • At HTT 1400°C, a silicon nitride broad peak (SiN4 and SiCN3) emerges from the massif. It appears as a shoulder near −20 ppm (SiC2N2). X-ray diffraction patterns do not provide similar information, owing to the amorphous organisation of the material. • At HTT 1500°C, the structure of the massif is more evident. Three more or less well-resolved peaks are observed which are respectively attributed to SiN4, SiCN3 and SiC2N2. A shoulder near −18 ppm seems to appear which can be silicon carbide. • At HTT 1600°C, crystallised silicon nitride (α and β) are observed, the proportion of which increases as initial C/N decreases. A silicon carbide massif (SiC4, SiC3N) is clearly separated from this one. Two significant samples, HMDS42 and HMDS44, are analysed in more detail using least square decomposition method, assuming different occupations sites as given in Figure 5.1.9. Results are shown on Figures 5.1.12 and 5.1.13. Table 5.1.5 gives the relative proportions of the different sites. Neither SiC4 nor SiC2N2 are observed till HTT is 1000°C. A mixture of such sites is observed at a higher temperature. From HTT 1550°C, crystallised SiN4 (α and β) sites are clearly identified. In the silicon carbide broad line, SiC4 and SiC3N sites are present. The relative proportions of crystallised silicon nitride clearly depend on the initial C/Nini composition (C/Nini = 0.73 and 0.57, respectively, for HMDS42 and HMDS44). Such different evolutions are shown on the chemical composition (Figure 5.1.14). An important remark concerns the duty cycle, that is, the time between two accumulations, to obtain reliable spectra. This time has to be of the order of five times that of the spin-lattice
Figure 5.1.12 Solid state 29Si MAS–NMR spectra at 99.36 MHz, rotation frequency of 5 kHz, of (a) HMDS42 and (b) HMDS44 heat-treated at 1000°C, 1400°C and 1500°C during 1 h in N atmosphere and decomposition, using a least square method, into different assumed Si environments (El Kortobi 1998).
< previous page
page_124
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_124.html [20/01/2010 10:04:23 AM]
page_125
< previous page
page_125
next page >
Page 125
Figure 5.1.13 Solid state 29Si MAS–NMR spectra at 99.36 MHz, rotation frequency of 5 kHz, of (a) HMDS42 and (b) HMDS44 heat-treated at 1550°C, 1600°C and 1700°C during 1 h in N atmosphere and decomposition, using a least square method, into different assumed Si environments (El Kortobi 1998). relaxation times of the species to observe. Figure 5.1.15 shows spectra obtained for different values of such time. One notices that the relative apparent proportion of silicon nitride is only significant for temperatures higher than 1550°C, which shows that the two massifs are associated with relatively short and long spinlattice relaxation times. Different authors, using MAS–NMR, had similarly used duty cycle as long as 30 mn to obtain reliable spectra (Dybowski et al. 1996). In the case considered here, it is necessary to reach 8000 s to estimate the relative proportion of silicon nitride in the different specimens. Amorphous silicon carbide massif relaxes more rapidly as shown in Figure 5.1.16. In Chapter 5.2, electron paramagnetic resonance (EPR) measurements show that the materials contain an important amount of paramagnetic centres. Besides, the study of the magnetisation as a function of the temperature as in the example on HMDS44 heat-treated at 1550°C, shows a Curie law dependence. This is in favour of localised paramagnetic centre organisation. As the above observation concerning the difference of spin-lattice relaxation times between silicon nitride and other species, it is obvious to consider that such centres are inside the amorphous silicon carbide structure. Same samples, HMDS42 and HMDS44, have been analysed using 13C MAS–NMR (Figure 5.1.17). The useful CP/MAS–NMR is useless in that temperature range, due to the lack of proton in the material. The difficulty in acquiring a good signal over noise spectra is related to the low-frequency measurement. This had been done to prevent side bands coming from a large CSA of the aromatic carbons. Different comments have to be made: • At HTT 1000°C, some differences are observable. A broad massif centred around −130 ppm is attributed to aromatic sp2 and oxygenated carbons. This is generally
< previous page
page_125
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_125.html [20/01/2010 10:04:24 AM]
page_126
< previous page
page_126
next page >
Page 126 Table 5.1.5 29Si chemical shift δ in ppm/TMS, obtained using a least square .tting method for HMDS42 and HMDS44 samples. Gaussian fit shape assumed for a theoretical decomposition of the experimental spectra. Δ is the Gaussian quadratic square deviation of each specie assumed HTT(° SiN4 SiCN3 SiC2N2 SiC3N SiC4 C) δ Δ %δ Δ %δ Δ % δ Δ % δ ö % (ppm) (ppm) (ppm) (ppm) (ppm) (ppm) (ppm) (ppm) (ppm) (ppm) HMDS42 1000 −53.6 18 67 −35 20 33 / / / / / / / / / 1400 −50 14 54 −34.6 13 30 −21 14 16 / / / / / / 1500 −48 14 34 −32 15 31 / / / / / / −14.5 15 35 1550 / / 9 / / / −21 8 6 −9 10 34.5 −17 8 31.5 1600 / / 13 / / / / / / −6 13 31.1 −18 10 56.5 1700 / / 10 / / / / / / −11 5 12.6 −17 6 74.4 HMDS44 1000 −53.6 17 80 −37 17 20 / / / / / / / / / 1400 −50 14 67 −36 14 16 −23 14 17 / / / / / / 1500 −53 12 40 −37 14 36 / / / / / / −20 13 24 1550 / / 48 / / / −22 7 5.5 −7 9 12.3 −17 10 34.2 1600 / / 40 / / / −23 5 6 −10 8.5 11.4 −17 8 42.6 1700 / / 42 / / / 21 6 3.2 −9 8 14.1 −17 6 40.8
< previous page
page_126
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_126.html [20/01/2010 10:04:24 AM]
page_127
< previous page
page_127
next page >
Page 127
Figure 5.1.14 Atomic chemical composition SiyCxNz (x + y + z = 1) of HMDS42 and HMDS44 as a function of heat treatment temperature. Arrows indicate evolution from as-formed to highest treatment temperature. considered as ‘free carbon’. Besides, for HMDS42, a small peak near −20 ppm can be attributed to sp3 Si bonded C. • From HTT 1400°C, the amount of Si bonded C increases, which is in accordance with the 29Si MAS–NMR observation. Besides, the existence of other environments such as CSixNy are possible. • At HTT 1550°C, the line around −20 ppm, related to silicon carbide, is more important for both samples. Although the difference is noticeable concerning the ‘free carbon’ still present in the richer C HMDS42 sample than in HMDS44, were it is now absent. More generally, similar determinations are of interest to characterise silicon carbide fibres and consequently their mechanical properties (Hommel et al. 1990; Laffon et al. 1989). Some comparisons can be done between the atomic chemical compositions and 29Si NMR determinations. From Table 5.1.5, with the relative proportions of SiN4(p), SiCN3(q), SiC2N2(r), SiC3N(s) and SiC4(t), it is possible to calculate the average atomic compositions SiyCxNz (x + y + z = 1) as a function of HTT and to plot Figure 5.1.18, using the following formula:
(5.2) The above values are listed in Table 5.1.6. Such obtained plots show a convergence of the two types of analysis at high heat temperature treatment of both samples. The divergence observed at low HTT originates from
< previous page
page_127
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_127.html [20/01/2010 10:04:25 AM]
page_128
< previous page
page_128
next page >
Page 128
Figure 5.1.15 Solid state 29Si MAS–NMR spectra obtained at different duty cycle (D1) values on HMDS44 and HMDS42, at different heat treatment temperatures. Spectra are adjusted so that the maximum of each spectrum is similar to the others. Signal over noise depends on the number of scans and consequently of the total time of accumulation, which is different for some spectra (El Kortobi 1998). an underestimation of C content. Those not being bonded to silicon C atoms are set in the amorphous ‘free carbon’ as it had been discussed above (Figure 5.1.17). This effect is not important for sample heat-treated at temperature higher than 1550°C, as it can be observed on the points corresponding to NMR measurements. They are in the vicinity of those in the chemical analysis. From the C content values obtained for chemical analysis and NMR, it is possible to estimate the proportion of ‘free carbon’ in total C. This calculation is only valid, within the experimental errors, in the temperature range 1000–1550°C (Figure 5.1.19). 5.1.3.2 Thermal evolution from NMR measurements This evolution can be roughly decomposed in three steps as follows: First step: HTT inferior to 1000°C This domain, from as-prepared powder till almost end of mineralisation, is mainly discussed in Chapter 2. The most efficient methods of
< previous page
page_128
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_128.html [20/01/2010 10:04:26 AM]
page_129
< previous page
page_129
next page >
Page 129
Figure 5.1.16 Solid state 29Si MAS–NMR spectra obtained at different duty cycle (D1) values on HMDS44 heat-treated at 1600°C (LB = 30 Hz, NS = 16) (El Kortobi 1998). characterisation are in particular TGA and IR. It is characterised by emission of H2O, NH3 and CH4. It results in the formation of Si N with ammoniac (Gérardin et al. 1997; Bowen 1980) and Si—C bonds with methane (Gérardin et al. 1997, Hasegawa and Okumura 1983) emissions. Second step: 1000–1500°C As seen from 29Si MAS–NMR, it starts with a rich nitrogen (N) to Si environment (SiN4, SiCN3) depending on the initial C/Nini concentration. Besides, 13C MAS–NMR demonstrate the presence of C not bonded to Si, named ‘free carbon’. The proportion of such C decreases considerably till 1500°C. Parallelly, it is observed as an increase of C to Si environment. Third step: 1550–1700°C The crystallisation of the material is observed, with important loss in weight due to the departure of N, consecutive to a carbo-reduction. Demixtion occurs with the appearance of wellcrystallised α − β SiN4 and of amorphous silicon carbides (SiC4, SiC3N and SiC2N2). 5.1.4 Pre-alloyed Si/C/N/Al/Y nanopowders In Chapter 7 explanations are given on the interest to use additives for the sintering of silicon nitride based materials. The objective here is to characterise nanosized ready-to-sinter powders including additives. Two types of additives have been incorporated: alumina (Al2O3) and yttria (Y2O3).
< previous page
page_129
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_129.html [20/01/2010 10:04:26 AM]
page_130
< previous page
page_130
next page >
Page 130
Figure 5.1.17 Solid state 13C MAS–NMR spectra at 25.15 MHz, rotation frequency of 5 kHz, of HMDS42 and HMDS44 at different heat treatment temperatures.
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_130.html (1 of 2) [20/01/2010 10:04:27 AM]
page_130
Figure 5.1.18 Atomic NMR and chemical compositions SiyCxNz (x + y + z = 1) of HMDS42 and HMDS44 as a function of heat-treated temperature. Arrows indicate evolution from as-formed to highest treatment temperature.
< previous page
page_130
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_130.html (2 of 2) [20/01/2010 10:04:27 AM]
page_131
< previous page
page_131
next page >
Page 131 Table 5.1.6 Atomic NMR composition CxSiyNz (x + y + z = 1) of HMDS42 and HMDS44 as a function of heat treatment temperature HTT(°C) C Si N HMDS42 1000 0.03896 0.4329 0.52814 1400 0.06987 0.43668 0.49345 1500 0.15315 0.45045 0.3964 1550 0.33175 0.47393 0.19431 1600 0.38462 0.48077 0.13462 1700 0.42157 0.4902 0.08824 HMDS44 1000 0.02155 0.43103 0.54741 1400 0.05652 0.43478 0.5087 1500 0.12796 0.47393 0.3981 1550 0.20354 0.44248 0.35398 1600 0.24658 0.45662 0.2968 1700 0.23767 0.44843 0.3139
Figure 5.1.19 ‘Free carbon’ evolution as a function of heat treatment temperature. Values are obtained owing to the formula: (xCA − xNMR)/xCA where xCA, xNMR are those of the chemical analysis and NMR, respectively. 5.1.4.1 Free carbon effect Samples HSAl03 and HSAl05, heat-treated from 1000°C to 1600°C in N atmosphere during 1 h, have been analysed using 29Si MAS–NMR (Figure 5.1.20). The following observations can be made: • From as-formed to HTT 1000°C, no important differences are observed. A broad peak around −20 ppm shows different environments of Si (SiC3N, SiC2N2 and/or SiC4). • At HTT 1400°C, a line narrowing is observed. Only SiC2N2 and/or SiC4 environments remain.
< previous page
page_131
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_131.html [20/01/2010 10:04:28 AM]
page_132
< previous page
page_132
next page >
Page 132
Figure 5.1.20 Solid state 29Si MAS–NMR spectra at 99.36 MHz, MAS speed of 5 kHz, of (a) HSAl03 and (b) HSAl05 at different heat treatment temperatures. At 1600°C, no silicon nitride remains; compare to Table 3.1.3 (El Kortobi 1998). • At HTT 1600°C, the narrowing is more important. A structure is perceptible, which can be attributed to α and β silicon carbide. 13C MAS–NMR is able to improve such results. Only as-formed samples can be analysed using CP and MAS. The sites are CH3Si and Si—CH2—Si in the range 0–5 ppm. • At HTT 1000°C, as hydrogen is expulsed with heat treatment, 13C MAS–NMR sp3 and sp2 C are observed. • From HTT 1400°C to 1600°C, the ‘free carbon’ massif disappears progressively. The line around 24 ppm is proportionally improved. This confirms the presence of partially crystallised silicon carbide (Figure 5.1.21). 27Al MAS–NMR shows three aluminium environments for as-formed materials. Tetra, penta and octahedral environments are observed (Figure 5.1.22). • At HTT 1000°C, such three sites are still observable, with a significant increase of the octahedral environment. • From HTT 1400°C to 1600°C, besides tetra and octahedral sites, there is a broad massif at lower field, around 90 ppm. This can be attributed, owing to measurements done on defined samples (AlON and SiAlON) (Figure 5.1.23), to aluminium oxynitrides AlOxN4−x, with 0 < x < 4 (Smith 1992; Mackenzie et al. 1994; Fitzgerald et al. 1994). At HTT 1400°C, this massif contains AlO3N and AlO2N2 (96 ppm), AlON3 (106 ppm) and AlN4 (114 ppm). At HTT 1600°C, the peak corresponding to AlN4 is easier to observe (Figure 5.1.24).
< previous page
page_132
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_132.html [20/01/2010 10:04:28 AM]
page_133
< previous page
page_133
next page >
Page 133
Figure 5.1.21 Solid state 13C MAS–NMR spectra at 25.15 MHz, rotation frequency of 5 kHz, of HSAl03 at different heat treatment temperatures (El Kortobi 1998).
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_133.html (1 of 2) [20/01/2010 10:04:29 AM]
page_133
Figure 5.1.22 Solid state 27Al MAS–NMR spectrum at 130.32 MHz of (a) HSAl03 and (b) HSAl05. MAS speed 12 kHz, 1 μs pulse, duty cycle 1 s, number of scans 600 (El Kortobi 1998).
< previous page
page_133
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_133.html (2 of 2) [20/01/2010 10:04:29 AM]
page_134
< previous page
page_134
next page >
Page 134
Figure 5.1.23 Solid state 27Al MAS–NMR spectrum at 130.32 MHz of different reference samples. MAS speed 12 kHz, 1 μs pulse, duty cycle 1s, number of scans 600. At 1600°C, N is bonded to aluminium; compare to Table 3.1.3. So, the following remarks can be made: • Al—O and A—N bonds are observed. • N, initially bonded to Si as SiC3N and SiC2N2, is finally bonded to aluminium oxynitrides AlOxN4−x. In conclusion, the study of the local environment of 13C,27 Al and 29Si nuclei, enables us to understand why, within the proportions of reactants used for the synthesis, such powders did not produce a compound suitable for sintering (Chapter 7). The large amount of ‘free carbon’ favours the nitridation of aluminium owing to the reaction: This aluminium nitridation is responsible for the N loss in the Si environment. A new series of preparation is done with hydrogen and ammonia added on. This is to obtain the trapping of reactive free radical •CH3. The 27Al spectra show that the aluminium nitridation is noticeably decreased (Figure 5.1.24). It presents an intense line at 60 ppm, attributed to AlO4, sharper than that observed in a glass or conventional sintered sample. This line corresponds to a well-organised tetrahedral specie, only surrounded by oxygen atoms. This should be an aluminium solid solution in β-SiAlON. Similarly, the 29Si spectra demonstrate the presence of silicon nitride (Figure 5.1.25). The comparison between samples prepared without (HSAl07) and with (HSAl09) ammonia (Figure 5.1.26) shows clearly this
< previous page
page_134
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_134.html [20/01/2010 10:04:29 AM]
page_135
< previous page
page_135
next page >
Page 135
Figure 5.1.24 Solid state 27Al MAS–NMR spectrum at 130.32 MHz of HSAl12 to HSAlY17. MAS speed 12 kHz, 1 μs pulse, duty cycle 1 s, number of scans 600. phenomenon not only for Si but also for aluminium. This support the analysis done above on the role of ‘free carbon’ effect which is clearly observable on 13C spectra (Figure 5.1.26). 5.1.4.2 Influence of hot pressing A comparison can be done between hot pressed and heat-treated nanopowders. As examples HSAl09 29Si and 27Al NMR measurements are shown in Figures 5.1.27 and 5.1.28. As the hot pressing had been done at a higher temperature than that of the nanopowder, silicon carbide has almost disappeared. The structured peak, corresponds to different silicon nitrides. As mentioned in Table 5.1.3, α- and β-Si3N4 respectively present a doublet and a singlet lines. Carduner et al. (1987) measured linewidth between 1.5 and 2.5 ppm (full-width at half-height) for well-crystallised material. Although the spectra are in accordance with these measurements, the decomposition, in order to have the relative proportion of β/ (α + β), is questionable. The powder heat treated at 1600°C is able to contain some amorphous part, which explains the higher intensity at −47 ppm. For the sintered powder, the β proportion estimation by X-ray diffraction is 30% (Table 7.6), which is qualitatively in accordance with the 29Si NMR observation. 27Al NMR spectra (Figure 5.1.27) show the AlxOyNz broad line with the typical peaks or shoulder characteristics of AlN4, AlO4 and AlO6 environments. A significant difference is observed with the relative proportions of the different species from one sample to another. This has to be compared with Figure 5.1.22 where alumina is bonded to variable environments containing N.
< previous page
page_135
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_135.html [20/01/2010 10:04:30 AM]
page_136
< previous page
page_136
next page >
Page 136
Figure 5.1.25 Solid state 29Si and 13C MAS–NMR spectra at 99.36 MHz and 125.76 MHz of HSAl14, HSAl15 heat treated at 1600°C/N2/1h.29Si MAS speed 5 kHz, 5.2 μs pulse, duty cycle 500 s, number of scans 38, 4; 13C MAS speed 5 kHz, 5 μs pulse, duty cycle 500 s, number of scans 244.
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_136.html (1 of 2) [20/01/2010 10:04:30 AM]
page_136
Figure 5.1.26 Solid state 29Si and 27Al MAS–NMR spectra at 99.36 MHz and 130.32 MHz of HSAl07, HSAl09 heat treated at 1600°C/N2/1 h. 29Si MAS speed 5 kHz, 5.2 μs pulse, duty cycle 500, 8000 s, number of scans 38, 121 and 4; 27Al MAS speed 14 kHz. 1.2 and 1 μs pulse, duty cycle 1 s, number of scans 3600. An underestimation of the amount silicon nitride is observed when a too short duty cycle is used (see Figure 5.15).
< previous page
page_136
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_136.html (2 of 2) [20/01/2010 10:04:30 AM]
page_137
< previous page
page_137
next page >
Page 137
Figure 5.1.27 Solid state 29Si MAS–NMR spectra at 99.36 MHz. MAS speed 5 kHz, 5.5 μs, duty cycle 8000 s, number of scans 10. Comparison between sintered and heat treated HSAl09 nanopowder.
Figure 5.1.28 Solid state 27Al MAS–NMR spectrum at 130.32 MHz. MAS speed 14 kHz, 1.2 μs pulse, duty cycle 1 s, number of scans 600. Comparison between sintered and heat treated HSAl09 nanopowder. 5.1.5 Conclusion The analyses of different nanopowders, as-prepared and heat treated at different temperature, show the efficiency of the solid-state NMR, particularly for not well-crystallised samples. The possibility of obtaining cross informations from different nuclei, as 13C,27Al and 29Si and eventually proton via CP will improve the structural analysis. This enables us to modify synthesis conditions as demonstrated on pre-alloyed Si/C/N/Al/ Y nanopowders.
< previous page
page_137
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_137.html [20/01/2010 10:04:31 AM]
page_138
< previous page
page_138
next page >
Page 138 References Apperley, D. C. Marshall, G. L. and Thompson, D. P. (1991) J. Am. Ceram. Soc., 74(4), 777. Bloch, F. (1958) Phys. Rev. 111, 841. Bowen, H. K. (1980) Mater. Sci., 44,1. Carduner, K. R., Blackwell, C. S., Hammond, W. B., Reidinger, F. and Hatfield, G. R. (1990) J. Am. Chem. Soc., 112, 4676. Carduner, K. R., Carter III, R. O., Milberg, M. E. and Crosbie, G. M. (1987) Anal. Chem., 59, 2794. Dando, N. R. and Tadayyoni, M. A. (1990) J. Am. Ceram. Soc., 73(8), 2242. Dybowsky, C., Gaffney, E. J., Sayir, A. and Rabinowitz, M. (1996) Colloids. Surf., A118, 171. El Kortobi, Youssef (1998) Thesis, Université P. M. Curie, Paris, France, http://corail.sudoc.abes.fr80 & SudocCatalogue no 053764552. Engelhardt, G. and Michel, D. (1987) High-resolution Solid-state NMR of Silicates and Zeolites, J. Wiley & Sons, New York. Finlay, G. R., Harman, J. S., Ricardson, M. F. and Williams, B. L. (1985) J. Chem. Soc., Chem. Commun., 159. Fitzgerald, J. J., Kohl, S. D. and Piedra, G. (1994) Chem. Mater., 6, 1915. Fyfe, C. A. (1983) Solid-state NMR for Chemists, C.F.C. Press Guelph. Gérardin, C., Taulelle, F. and Bahloul, D. (1997) J. Mater. Chem., 7(1), 117. Guth, J. R. and Petuskey, W. T. (1987) J. Phys. Chem., 91(20), 5361. Harris, R. K., Leach, M. J. and Thompson, D. P. (1990) Chem. Mater., 2, 320. Hartman, J. S., Richardson, M. F., Sherriff, B. and Winsborrow, B. G. (1987) J. Am. Soc., 109, 6059. Hasegawa, Y. and Okamura, K. (1983) J. Mater. Sci., 18, 3633. Hockey, J. A. (1965) Chem. Ind. (London) 57. Hommel, H., Miquel, J. L. and Legrand, A. P. (1990) L’Industrie Céramique, 849,5. Laffon, C., Flank, A. M., Lagarde, P., Laridjani, M., Hagege, R., Olry, P., Cotteret, J., Dixmier, J., Miquel, J. L., Hommel, H. and Legrand, A. P. (1989) J. Mater. Sci., 24, 1503. Lippmaa, E. and Samoson, A. (1982) Bruker Rep., 1,6. Lippmaa, E., Magi, M., Samoson, A., Engelhardt, G. and Grimmer, A. R. (1982) J. Am. Chem. Soc., 102, 4899. Mackenzie, K. J. D., Meinhold, R. H., White, G. V., Sheppard, C. M. and Sherriff, B. L. (1994) J. Mater. Sci., 29, 2611. Marsman H. (1981) NMR Basic Principles and Progress, 17 (eds P. Diehl, E. Fluck and R. Kosfeld), SpringerVerlag Berlin, p. 65. Müller, K. (1999) Precursor-derived Ceramics (eds J. Bill, F. Wakai and F. Aldinger), Wiley-VCH. Richardson, M. F., Hartman, J. S., Guo, D. and Winsborrow, B. G. (1992) Chem. Mater., 4, 318. Samoson, A. and Lippmaa, E. (1983) Phys. Rev., B28, 6567. Schmidt, W. R., Interrante, L. V., Doremus, R. H., Trout, T. K., Marchetti, P. S. and Maciel, G. E. (1991) Chem. Mater., 3, 257. Seitz, J., Bill, J., Egger, N. and Aldinger, F. (1996) J. Eur. Ceram. Soc., 16, 885. Smith, M. E. (1992) J. Phys. Chem., 96, 1444. Tateyama, H., Noma, H., Adashi, Y. and Komatsu, M. (1997) Chem. Mater., 9, 766. Templin, M., Friedrich, U., Wiesner, U. and Spiess, H. W. (1999) Precursor-derived Ceramics (eds J. Bill, F. Wakai and F. Aldinger), Wiley-VCH. Tougne, P., Hommel, H., Legrand, A. P., Herlin, N., Luce, M. and Cauchetier, M. (1993) Diamond Relat. Mater., 2, 486. Tuel, A., Hommel, H., Legrand, A. P., Chevallier, Y. and Morawski, J.C. (1990) Colloids. Surf., 45, 413. Vercedia, G., O’Brien, K. L., Schmidt, W. R. and Apple, T. M. (1998) Chem. Mater., 10, 1003. Wagner, G. W., Na, B. -K. and Vannice, M. A. (1989) J. Phys. Chem., 93, 5061. Wakai, F., Kodama, Y., Sakaguchi, S., Murayama, N., Izaki, K. and Niihara, K. (1990) Lett. Nature, 344, 421.
< previous page
page_138
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_138.html [20/01/2010 10:04:32 AM]
page_139
< previous page
page_139
next page >
Page 139 5.2 Paramagnetic defect states in silicon-based nanopowders Abdelhadi Kassiba and Stéphane Charpentier 5.2.1 Introduction Electron paramagnetic resonance (EPR) technique is a suitable tool in characterising the paramagnetic defects in the Si/C/N nanopowders. The EPR experiments are carried out both following the annealing temperature (realised separately up to 1800°C) and the specimen temperature (in situ from 4 to 1000 K). Different EPR frequency bands (4–95 GHz) and numerical EPR spectrum analyses are needed for an understanding of the defect nature and properties. However, when mixed compositions and structures coexist as in (Si/C/N) networks, the overlapping of the resonance lines leads to structureless EPR spectra. In such materials, it is possible to assess the concentration of paramagnetic defects and their properties such as being localised or delocalised. More quantitative analyses can be achieved on more homogeneous materials (Si/C) where structured EPR spectra are obtained. Precise insights on the paramagnetic defects are made and correlated with the material composition, structure and physical properties. The first set of investigations is devoted to SiC nanopowders synthesised by a laser pyrolysis of a gaseous mixture (SiH4, C2H2). The batches, referred as SiC242, SiC163 and SiC177, differ by the residence time of the reactants in the laser beam and by the gaseous precursor flux rate [SiH4]/[C2H2]. The defect concentration is relatively high in all the samples (NS ≈ 1020 spin g−1) and their nature seems correlated with the coexisting SiC polytypes. A consistent numerical analysis of the EPR spectra, over several EPR frequencies, was developed in order to identify the paramagnetic centres. Whatever the annealing stage and the EPR frequency band, three paramagnetic defects with well-defined ( , ) tensors coexist with contributions dependent on the annealing stages. Delocalised centres, thermally induced by varying the sample temperature, are also evidenced in these nanopowders. They would contribute to the significant electric conduction induced by annealing at Ta ≥ 1500°C. The second deals with Si/C/N materials (referred as HMDS40–45) where the coexisting structures (SiC, Si3N4) and the free carbon (C) content give rise to a large unpaired spin concentration brought by two types of paramagnetic centres. Their contributions depend on the synthesis conditions and on the annealing stages. We have shown that the rate of C on nitrogen (N) monitors the defect concentration and the annealing under N partial pressure (nitriding process) favours the creation of unpaired spins in the Si3N4-rich powders. The forthcoming EPR investigations focus on these two classes of silicon-based nanomaterials.
< previous page
page_139
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_139.html [20/01/2010 10:04:32 AM]
page_140
page_140
< previous page
next page >
Page 140 5.2.2 Theoretical background Paramagnetic defects in these Si/C/N covalent networks, consist mainly in unpaired electrons. Under an , each paramagnetic defect is described by an effective spin Hamiltonian which
external magnetic field reads:
where β represents the Bohr magneton, k refers to an interacting nucleus (nuclear spin Ik) with hyperfine diagonal tensor in a reference frame (xk, yk, zk) centred on the (k) nuclei. The tensor, has a diagonal form in its principal (magnetic) frame (X Y Z), with components in the order of ge = 2.0023 value; that is, is defined by angular variables the free electron Landé factor. In crystalline powders, the magnetic field (θ0, φ0) with respect to the magnetic axes (X, Y, Z). The local resonance fields Bres; that is, the EPR line position, is expressed as follows:
where h is the Planck’s constant and νEPR = 9.5 GHz in X-band EPR measurements. Be is the resonance position of a free electron. The EPR signal of paramagnetic defects would have the shape of a continuous absorption background with singularities at the positions
However, in current EPR experiments the derivative of the absorption line is recorded. The small departure Δgi = gi − ge, in a given (i = X, Y, Z) direction, results from a weak spin–orbit coupling (λ · the perturbation formula:
·
) through
and represent respectively the ground and the excited electronic states of energies E(0) and where E(n). Quantitative analysis of the tensor components cannot be undertaken safely in these heterogeneous Si/C/N media. However, the evolution of Δg shifts with particular thermal treatments that can be used to characterise the changes of the local environments around the involved paramagnetic centres. With regard to the hyperfine tensor components , they are determined experimentally from the hyperfine line positions. A brief theoretical justification of these parameters can be established in the following simple case. When the electronic spin density on the nuclei exhibits an axial symmetry around the zk-axis, the components of the
tensor are:
with
< previous page
page_140
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_140.html [20/01/2010 10:04:33 AM]
page_141
< previous page
page_141
next page >
Page 141
Aiso represents the contact interaction parameter and Aaniso accounts for a dipolar interaction.
and
represent the orbital wave function of (s) and (p) types related to the (k) ion. (r, θ) are the radial and azimuthal coordinates of the unpaired electron in the reference frame centred on the nucleus. gn and βn represent respectively the nuclear g-factor and the nuclear Bohr magneton. The hyperfine lines are observed when the unpaired electron interacts with a nuclear spin in its near environment. For Si/C/N materials, the nuclear spin (I) is brought by 13C by 29Si or by 14N (I = 1, na = 99.6%). The intensity and the number of the hyperfine lines can be used to determine the nature of the interacting nuclei. Moreover, the integrated intensity of the EPR signal is proportional to the paramagnetic defect concentration (Ns) and to their magnetic susceptibility (χ). The temperature dependence of χ informs on the localised or delocalised nature of the paramagnetic species. Indeed, when χ varies with temperature following the Curie law (χ = C/T ), the unpaired electrons are localised in the host material sites. In the case of delocalised unpaired electrons, χ is temperature independent and ‘Pauli-like’ paramagnetism is expected. 5.2.3 Experimental details EPR experiments are carried out on Brucker spectrometer with different frequency bands [S(4 GHz), X (10 GHz), K (24 GHz), Q (34 GHz) and W (95 GHz)]. Investigations at different temperatures (4–300 K) are conducted on an Oxford cryostat. The high unpaired spin concentration in the samples limits the microwave power below 2 mW and the modulation field to 0.5 G. Saturation phenomena and EPR line shape distortions are thus avoided. The absolute concentration (Ns) of paramagnetic species is determined by a comparison with CuSO4 · 5H2O single crystal (≈3·1021 spin g−1). This absolute Ns estimate is within a range of four times more or less than the real value. 5.2.4 Si/C powders Three Si/C batches (SiC163, SiC177 and SiC212) synthesised from gaseous precursors (Table 2.2) are investigated. Whatever the nanopowder series are, the EPR spectra have common features and similar electrical properties. So, the forthcoming report is limited to the SiC212 batch referred below as SiC212 1200– 1800°C according to annealing temperature T = 1200–1800°C. The structural modifications, the powder composition and grain morphology are well known (Charpentier 1997, 1999 and 1999a). Figure 5.2.1(a) shows the room temperature EPR spectra at X-band in the SiC212 1200°C and 1650°C samples. High temperature measurements in the SiC212 1200°C sample up to 600°C under air did not show any change on the EPR spectrum features except for the obvious intensity decrease. The reversible behaviour of the EPR spectra, that is, before and after the oxidation rules out any influence of the oxidation process or thermal removal of the paramagnetic species. Furthermore, it seems that the defects are not connected with hydrogen which may be released by annealing at high temperatures. The defects are intrinsic to the material mainly caused by vacancies in the C or silicon (Si) sites of the coexisting C arrangements and SiC polytypes. Low temperature measurements are needed in order to assess the localised or delocalised nature of the defects. In the SiC212 1200°C sample, the X-band EPR spectrum is drastically
< previous page
page_141
next page >
file:///C|/Users/steppenwolf/Documents/education/books/to%20burn/nanocomposites/files/page_141.html [20/01/2010 10:04:34 AM]
page_142
< previous page
page_142
next page >
Page 142
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_142.html (1 of 2) [20/01/2010 10:04:34 AM]
page_142
Figure 5.2.1 (a) Typical X-band EPR spectra in SiC212 nanomaterials annealed at 1200°C and 1650°C. (b) Evolution of the SiC212 1200°C EPR spectrum with the temperature. (c) Experimental and calculated W-band EPR spectra in the SiC212 1200°C sample. The contributions from the different paramagnetic centres are also shown (relative contributions to the EPR spectrum DI: 21%; DII 49%; DIII 30%).
< previous page
page_142
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_142.html (2 of 2) [20/01/2010 10:04:34 AM]
page_143
< previous page
page_143
next page >
Page 143
Figure 5.2.2 Evolution with the temperature of the EPR signal integrated intensity weighted by T: (a) in the SiC212 1200°C sample and (b) in the SiC212 1600°C sample. broadened by lowering the temperature (Figure 5.2.1(b)). This is understood by the possible defect motion which is frozen at low temperature. A double integration of the EPR signal allows the determination of the overall intensity which is proportional to the spin susceptibility χ (Figure 5.2.2). A departure of χ(T) from the Curie law above 150 K, also observed in the SiC212 1650°C sample (Figure 5.2.2), indicates the presence of delocalised paramagnetic species. Furthermore, the peak-shaped behaviour of the product χ(T) × T around 30 K is consistent with a localisation of the defects and correlated unpaired spins. Consistent numerical analyses of the EPR spectra are hereafter conducted in order to determine the paramagnetic defect features in these SiC nanopowders. The paramagnetic centres are S = 1/2-defects file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_143.html (1 of 2) [20/01/2010 10:04:35 AM]
page_143
assumed to interact with p equivalent nuclei (nuclear spin
< previous page
page_143
next page >
file:///C|/Users/steppenwolf/Documents/educatio...ks/to%20burn/nanocomposites/files/page_143.html (2 of 2) [20/01/2010 10:04:35 AM]
page_144
< previous page
page_144
next page >
Page 144 . Under an applied magnetic field
, the spin Hamiltonian is given by:
represents the hyperfine coupling tensor between the electronic and nuclear spins. The magnetic dipole transition intensitie