Deutsche Forschungsgemeinschaft Macromolecular Systems: Microscopic Interactions and Macroscopic Properties
Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
Deutsche Forschungsgemeinschaft Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Final report of the collaborative research centre 213, ``Topospezifische Chemie und Toposelektive Spektroskopie von MakromolekÏlsystemen: Mikroskopische Wechselwirkung und Makroskopische Funktion'', 1984^1995 Edited by Heinz Hoffmann, Markus Schwoerer and Thomas Vogtmann Collaborative Research Centres
Deutsche Forschungsgemeinschaft Kennedyallee 40, D-53175 Bonn, Federal Republic of Germany Postal address: D-53175 Bonn Phone: ++49/228/885-1 Telefax: ++49/228/885-2777 E-Mail: (X.400): S = postmaster; P = dfg; A = d400; C = de E-Mail: (Internet RFC 822):
[email protected] Internet: http://www.dfg.de
This book was carefully produced. Nevertheless, editors, authors and publisher do not warrant the information contained therein to be free of errors. Readers are advised to keep in mind that statements, data, illustrations, procedural details or other items may inadvertently be inaccurate.
Library of Congress Card No.: applied for
A catalogue record for this book is available from the British Library.
Die Deutsche Bibliothek – CIP Cataloguing-in-Publication Data A catalogue record for this publication is available from Die Deutsche Bibliothek ISBN 3-527-27726-9
WILEY-VCH Verlag GmbH, D-69469 Weinheim (Federal Republic of Germany), 2000 Printed on acid-free and chlorine-free paper All rights reserved (including those of translation into other languages). No part of this book may be reproduced in any form – by photoprinting, microfilm, or any other means – nor transmitted or translated into machine language without written permission from the publishers. Registered names, trademarks, etc. used in this book, even when not specifically marked as such, are not to be considered unprotected by law. Cover Design and Typography: Dieter Hüsken Composition: ProSatz Unger, D-69469 Weinheim Printing: betz-druck gmbh, D-64291 Darmstadt Bookbindung: J. Schäffer GmbH & Co. KG, D-67269 Grünstadt Printed in the Federal Republic of Germany
Contents
Preface . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
XV
List of Contributors . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . XVII
I
Mainly Solids
1
Model Systems for Photoconductive Material . . . . . . . Harald Meyer and Dietrich Haarer Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental techniques . . . . . . . . . . . . . . . . . . . . . . . . Transport models . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Results . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Moleculary doped polymers . . . . . . . . . . . . . . . . . . . . . . Side-chain polymers . . . . . . . . . . . . . . . . . . . . . . . . . . . Conjugated systems . . . . . . . . . . . . . . . . . . . . . . . . . . . . Outlook . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
.............. ... ... ... ... ... ... ... ... ...
3 4 5 7 7 9 10 12 13
Novel Photoconductive Polymers . . . . . . . . . . . . . . . . . Jörg Bettenhausen and Peter Strohriegl Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Liquid crystalline oxadiazoles and thiadiazoles . . . . . . . . The basic idea . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Monomer synthesis . . . . . . . . . . . . . . . . . . . . . . . . . . . . Oligo- and polysiloxanes with pendant oxadiazole groups Photoconductivity measurements . . . . . . . . . . . . . . . . . . Starburst oxadiazole compounds . . . . . . . . . . . . . . . . . . . Motivation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Synthesis of starburst oxadiazole compounds . . . . . . . . . Thermal properties . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
..............
15
........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ...........
15 16 16 17 19 21 22 22 24 27 30
1.1 1.2 1.3 1.4 1.4.1 1.4.2 1.4.3 1.5
2 2.1 2.2 2.2.1 2.2.2 2.2.3 2.2.4 2.3 2.3.1 2.3.2 2.3.3
........... ........... ........... ........... ........... ........... ........... ........... ...........
... ... ... ... ... ... ... ... ... ... ...
3
V
Contents 3 3.1 3.2 3.3 3.4 3.5
4
4.1 4.2 4.2.1 4.2.2 4.2.3 4.2.4 4.3 4.4 4.4.1 4.4.2 4.4.3 4.5
5 5.1 5.2 5.3 5.4 5.5
6
6.1 6.2 6.3 6.4
VI
Theoretical Aspects of Anomalous Diffusion in Complex Systems . . . Alexander Blumen General aspects . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Photoconductivity . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The Matheron-de-Marsily model . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Polymer chains in MdM flow fields . . . . . . . . . . . . . . . . . . . . . . . . . . . Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Acknowledgements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
...
31
... ... ... ... ... ... ...
31 32 36 38 42 42 43
...
44
... ... ... ... ... ... ... ... ... ... ... ... ... ...
44 46 46 47 49 52 54 55 55 58 62 65 66 66
Spectral Diffusion due to Tunneling Processes at very low Temperatures Hans Maier, Karl-Peter Müller, Siegbert Jahn, and Dietrich Haarer Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The optical cryostat . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Theoretical considerations . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Temperature dependence . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Time dependence . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
68
Low-Temperature Heat Release, Sound Velocity and Attenuation, Specific Heat and Thermal Conductivity in Polymers . . . . . . . . . . . . Andreas Nittke, Michael Scherl, Pablo Esquinazi, Wolfgang Lorenz, Junyun Li, and Frank Pobell Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Phenomenological theory for heat release . . . . . . . . . . . . . . . . . . . . . . . Generalities . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The standard tunneling model with infinite cooling rate . . . . . . . . . . . . Influence of higher-order tunneling processes and a finite cooling rate . The influence of a constant and thermally activated relaxation rate . . . . Experimental details . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental results and discussion . . . . . . . . . . . . . . . . . . . . . . . . . . . Specific heat and thermal conductivity . . . . . . . . . . . . . . . . . . . . . . . . . Internal friction and sound velocity . . . . . . . . . . . . . . . . . . . . . . . . . . . Heat release . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Acknowledgements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
Optically Induced Spectral Diffusion in Polymers Containing Water Molecules: A TLS Model System . . . . . . . . . . . . . . . . . . . . . . . . . . . . Klaus Barth, Dietrich Haarer, and Wolfgang Richter Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental setup for burning and detecting spectral holes . . . . . . . . . Reversible line broadening phenomena . . . . . . . . . . . . . . . . . . . . . . . . . Induced spectral diffusion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
68 69 71 73 74 76
...
78
... ... ... ... ...
78 79 80 83 87
Contents 7 7.1 7.2 7.2.1 7.2.2 7.2.3 7.2.4 7.3 7.3.1 7.3.2 7.3.3 7.4
8
8.1 8.2 8.3 8.4 8.5
9
9.1 9.2 9.2.1 9.2.2 9.2.3 9.2.3.1 9.2.3.2 9.2.3.3 9.2.4 9.3 9.3.1 9.3.2 9.3.3 9.3.4 9.3.5 9.3.6 9.3.7
Slave-Boson Approach to Strongly Correlated Electron Systems . . . . Holger Fehske, Martin Deeg, and Helmut Büttner Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Slave-boson theory for the t-t'-J model . . . . . . . . . . . . . . . . . . . . . . . . . SU(2)-invariant slave-particle representation . . . . . . . . . . . . . . . . . . . . . Functional integral formulation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Saddle-point approximation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Magnetic phase diagram of the t-t'-J model . . . . . . . . . . . . . . . . . . . . . Comparison with experiments . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Normal-state transport properties . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Magnetic correlations and spin dynamics . . . . . . . . . . . . . . . . . . . . . . . Inelastic neutron scattering measurements . . . . . . . . . . . . . . . . . . . . . . . Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
...
88
... ... ... ... ... ... ... ... ... ... ... ...
88 90 90 93 95 97 102 102 105 106 109 110
...
113
... ... ... ... ... ... ...
113 114 116 117 119 120 120
..............
122
........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ...........
122 129 129 131 131 131 136 139 141 144 145 147 149 150 152 152 154
Non-Linear Excitations and the Electronic Structure of Conjugated Polymers . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Klaus Fesser Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Models . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Disorder . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Non-linear excitations . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Perspective . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Acknowledgements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Diacetylene Single Crystals . . . . . . . . . . . . . . . . . . . . . Markus Schwoerer, Elmar Dormann, Thomas Vogtmann, and Andreas Feldner Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Photopolymerization . . . . . . . . . . . . . . . . . . . . . . . . . . . Carbenes . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Intermediate photoproducts . . . . . . . . . . . . . . . . . . . . . . Electronic structure of dicarbenes . . . . . . . . . . . . . . . . . . Electron spin resonance of quintet states (5DCn) . . . . . . ENDOR of quintet states . . . . . . . . . . . . . . . . . . . . . . . . ESR and ENDOR of triplet dicarbenes 3DCn . . . . . . . . . Flash photolysis and reaction dynamics of diradicals . . . . Holography . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Theory . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental setup . . . . . . . . . . . . . . . . . . . . . . . . . . . . General characterization . . . . . . . . . . . . . . . . . . . . . . . . Angular selectivity . . . . . . . . . . . . . . . . . . . . . . . . . . . . Prepolymerized samples . . . . . . . . . . . . . . . . . . . . . . . . . Chain length, polymer profile, and grating profiles . . . . . Multrecording . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ...
VII
Contents 9.3.8 9.4 9.4.1 9.4.1.1 9.4.1.2 9.4.1.3 9.4.2 9.4.2.1 9.4.2.2 9.4.2.3 9.4.2.4 9.4.3 9.4.4 9.5 9.5.1 9.5.2 9.5.3 9.5.4 9.5.5 9.5.6 9.5.7 9.5.8 9.5.9 9.5.10
Holography . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Di-, pyro-, and ferroelectricity . . . . . . . . . . . . . . . . . . . . Dielectric properties of diacetylenes . . . . . . . . . . . . . . . . Correlation of polymer content and electric permittivity . Application to topospecifically modified diacetylenes . . . Additional applications . . . . . . . . . . . . . . . . . . . . . . . . . Pyroelectric diacetylenes . . . . . . . . . . . . . . . . . . . . . . . . IPUDO . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . NP/4-MPU . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . DNP/MNP . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Spurious piezo and pyroelectricity of diacetylenes . . . . . . The ferroelectric diacetylene DNP . . . . . . . . . . . . . . . . . Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Non-linear optical properties . . . . . . . . . . . . . . . . . . . . . Aims of investigation . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental setup . . . . . . . . . . . . . . . . . . . . . . . . . . . . Theoretical approaches . . . . . . . . . . . . . . . . . . . . . . . . . Sample preparation . . . . . . . . . . . . . . . . . . . . . . . . . . . . Value and phase of the third order susceptibility w(3) . . . . Relaxation of the singlet exciton . . . . . . . . . . . . . . . . . . The w(3) tensor components . . . . . . . . . . . . . . . . . . . . . . Signal saturation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Spectral dispersion, phase, and relaxation of w(5) . . . . . . . Conclusion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ...........
... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ...
154 155 156 156 158 159 159 159 160 161 161 162 166 167 167 167 170 170 170 171 172 173 174 176 177
10
...
181
10.1 10.2 10.3 10.4 10.5 10.6 10.7 10.8
Matrix-Molecule Interaction in Dye-Doped Rare Gas Solids . . . . . . . Thomas Giering, Peter Geißinger, Wolfgang Richter, and Dietrich Haarer Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Stochastic theory . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Rare gases . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Inhomogeneous absorption lines . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Pressure effects . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Rare gas mixtures . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Acknowledgements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
... ... ... ... ... ... ... ... ... ...
181 183 186 187 188 190 191 194 195 195
II
Mainly Micelles, Polymers, and Liquid Crystals
11
The Micellar Structures and the Macroscopic Properties of Surfactant Solutions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Heinz Hoffmann General behaviour of surfactants . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
11.1 VIII
199 199
Contents 11.2 11.3 11.3.1 11.3.2 11.3.3 11.4 11.4.1 11.4.2 11.4.3 11.4.4 11.5 11.5.1 11.5.2 11.5.3 11.5.4 11.6 11.6.1 11.6.2 11.6.3 11.6.4 11.7 11.7.1 11.7.2 11.8 11.9
From globular micelles towards bilayers . . . . . . . . . . . . . . . . . . . . . . . . Viscoelastic solutions with entangled rods . . . . . . . . . . . . . . . . . . . . . . General behaviour . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Viscoelastic systems . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Mechanisms for the different scaling behaviour . . . . . . . . . . . . . . . . . . Viscoelastic solutions with multilamellar vesicles . . . . . . . . . . . . . . . . . The conditions for the existence of vesicles . . . . . . . . . . . . . . . . . . . . . Freeze fracture electron microscopy . . . . . . . . . . . . . . . . . . . . . . . . . . . Rheological properties . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Model for the shear modulus . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Ringing gels . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The aminoxide system . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The bis-(2-ethylhexyl)sulfosuccinate system . . . . . . . . . . . . . . . . . . . . . PEO-PPO-PEO block copolymers . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Lyotropic mesophases . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Nematic phases and their properties . . . . . . . . . . . . . . . . . . . . . . . . . . . Cholesteric phases and their properties . . . . . . . . . . . . . . . . . . . . . . . . . Vesicle phases and L3 phases . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Shear induced phenomena . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . General . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Under what conditions do we find drag-reducing surfactants? . . . . . . . . SANS measurements on micellar systems . . . . . . . . . . . . . . . . . . . . . . . A new rheometer . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ...
200 202 202 205 209 211 211 212 213 217 220 220 221 224 226 227 227 228 232 233 236 236 236 239 243 247
12
Photophysics of J Aggregates . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Hermann Pschierer, Hauke Wendt, and Josef Friedrich Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Basic aspects of pressure and electric field phenomena in hole burning spectroscopy of J aggregates . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Results . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Discussion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Pressure phenomena . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Electric field-induced phenomena . . . . . . . . . . . . . . . . . . . . . . . . . . . . Acknowledgements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
...
251
...
251
... ... ... ... ... ... ... ...
252 253 254 256 256 258 258 259
..............
260
........... ........... ........... ...........
260 264 264 266
12.1 12.2 12.3 12.4 12.5 12.5.1 12.5.2
13 13.1 13.2 13.2.1 13.2.2
Convection Instabilities in Nematic Liquid Crystals . . Lorenz Kramer and Werner Pesch Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Basic equations and instability mechanisms . . . . . . . . . . The director equation . . . . . . . . . . . . . . . . . . . . . . . . . . . The velocity field . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
... ... ... ...
IX
Contents 13.2.3 13.2.3.1 13.2.3.2 13.2.4 13.3 13.4 13.5 13.5.1 13.5.2 13.5.3 13.5.3.1 13.5.3.2 13.6
Electroconvection . . . . . . . . . . . . . . . . . . . The standard model . . . . . . . . . . . . . . . . . . The weak electrolyte model . . . . . . . . . . . . Rayleigh-Bénard convection . . . . . . . . . . . . Theoretical analysis . . . . . . . . . . . . . . . . . . Rayleigh-Bénard convection . . . . . . . . . . . . Electrohydrodynamic convection . . . . . . . . Linear theory and type of bifurcation . . . . . Results of Ginzburg-Landau equation . . . . . Beyond the Ginzburg-Landau equation . . . . Experimental results . . . . . . . . . . . . . . . . . Theoretical results and discussion . . . . . . . . Concluding remarks . . . . . . . . . . . . . . . . . . Acknowledgements . . . . . . . . . . . . . . . . . . Note added . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . .
14
Preparation and Properties of Ionic and Surface Modified Micronetworks . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Michael Mirke, Ralf Grottenmüller, and Manfred Schmidt Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Polymerization in normal microemulsion . . . . . . . . . . . . . . . . . . . . . . . Mechanism and size control . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Surface functionalization of microgels . . . . . . . . . . . . . . . . . . . . . . . . . Polymerization in inverse microemulsion . . . . . . . . . . . . . . . . . . . . . . . Preparation of ionic microgels . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Properties of ionic microgels and interparticle interaction . . . . . . . . . . . Conclusion and relevance to future work . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
14.1 14.2 14.2.1 14.2.2 14.3 14.3.1 14.3.2 14.4
15
15.1 15.2 15.2.1 15.2.2 15.2.3 15.2.3.1 15.2.3.2 15.2.4 15.3 15.3.1 15.3.2 15.3.2.1 15.3.2.2 X
.......... .......... .......... .......... .......... .......... .......... .......... .......... .......... .......... .......... .......... .......... .......... ..........
........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ...........
Ferrocene-Containing Polymers . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Oskar Nuyken, Volker Burkhardt, Thomas Pöhlmann, Max Herberhold, Fred Jochen Litterst, and Christian Hübsch Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Addition polymers . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Radical polymerization . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Radical copolymerization . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Anionic polymerization of VFc . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Living polymerization . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Block copolymers . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Polymeranalogeous reactions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Polymers with ferrocene units in the main chain . . . . . . . . . . . . . . . . . . Polycondensation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Polymers by addition of dithiols to diolefins . . . . . . . . . . . . . . . . . . . . . Radical reaction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Base catalyzed reactions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ...
267 267 268 269 269 275 278 278 279 281 281 282 286 288 289 290
...
295
... ... ... ... ... ... ... ... ...
295 295 295 298 299 299 299 303 304
...
305
... ... ... ... ... ... ... ... ... ... ... ... ...
305 306 306 308 308 309 312 314 315 315 316 316 316
Contents 15.3.2.3 15.3.3 15.3.4 15.4
Acid catalyzed reactions . . . . . . . . . . . . . . . . . . . . . . . . 1,1'-dimercapto-ferrocene as initiator . . . . . . . . . . . . . . . Reductive coupling . . . . . . . . . . . . . . . . . . . . . . . . . . . . Mößbauer studies of polymers containing ferrocene . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
........... ........... ........... ........... ...........
... ... ... ... ...
318 319 320 320 323
16
Transfer of Vibrational Energy in Dye-Doped Polymers . . . . . . . . . . Johannes Baier, Thomas Dahinten, and Alois Seilmeier Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Results and discussion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
...
325
... ... ... ... ...
325 326 327 332 332
...
333
... ... ... ... ... ... ... ... ... ...
333 334 337 337 337 339 341 342 343 343
..............
344
........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ........... ...........
344 344 344 345 345 346 346 346 347 348 348 348 349 350 350 352
16.1 16.2 16.3 16.4
17
17.1 17.2 17.3 17.4 17.4.1 17.4.2 17.4.3 17.4.4 17.5
18 18.1 18.1.1 18.1.2 18.1.3 18.1.4 18.1.5 18.2 18.2.1 18.2.2 18.2.3 18.3 18.3.1 18.3.2 18.4 18.4.1 18.4.2
Picosecond Laser Induced Photophysical Processes of Thiophene Oligomers . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Dieter Grebner, Matthias Helbig, and Sabine Rentsch Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Experimental . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Spectroscopic properties of oligothiophenes . . . . . . . . . . . . . . . . . . . . . Results . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Picosecond-transient spectra of oligothiophenes in solution . . . . . . . . . . Time behaviour of transient spectra . . . . . . . . . . . . . . . . . . . . . . . . . . . Size dependence of spectroscopic properties of oligothiophenes . . . . . . Size dependence of the kinetic behaviour of oligothiophenes . . . . . . . . . Discussion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Topospecific Chemistry at Surfaces . . . . . . . . . . . . . . . Hans Ludwig Krauss Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The problem . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Preparative and analytical methods . . . . . . . . . . . . . . . . . Industrial applications . . . . . . . . . . . . . . . . . . . . . . . . . . The standard procedures of the Phillips process . . . . . . . Earlier work . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The support . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Unmodified silica . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Modified silica . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Others . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Transition metal surface compounds . . . . . . . . . . . . . . . . The metals . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Impregnation and activation . . . . . . . . . . . . . . . . . . . . . . Coordinatively unsaturated sites . . . . . . . . . . . . . . . . . . . Reduction of saturated surface compounds . . . . . . . . . . . Elimination of ligands . . . . . . . . . . . . . . . . . . . . . . . . . .
... ... ... ... ... ... ... ... ... ... ... ... ... ... ... ...
XI
Contents 18.5 18.5.1 18.5.2 18.6 18.6.1 18.6.2 18.6.3 18.7 18.8
Physical properties of the coordinatively unsaturated sites . . . . . . . . . . . Topologically different sites . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Optical and magnetic properties . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Chemical properties of the coordinatively unsaturated sites . . . . . . . . . . Survey of catalytic reactions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Olefin polymerization . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Other catalytic reactions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Deactivation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Summary and outlook . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
... ... ... ... ... ... ... ... ... ...
353 353 353 355 355 356 360 361 362 363
III
Biopolymers
Site-Directed Spectroscopy and Site-Directed Chemistry of Biopolymers Stefan Limmer, Günther Ott, and Mathias Sprinzl 19.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 19.2 Site-specific NMR spectroscopy of chemically synthesized RNA duplexes . . 19.2.1 Stability of tRNA-derived acceptor stem duplexes . . . . . . . . . . . . . . . . . . . . 19.2.2 Manganese ion binding sites at RNA duplexes . . . . . . . . . . . . . . . . . . . . . . 19.2.3 Structural determination of short RNA duplexes by 2D NMR spectroscopy . 19.2.4 NMR derived model of the tRNAAla acceptor arm . . . . . . . . . . . . . . . . . . . 19.2.5 Chemical shifts and scalar coupling as an indicator of RNA structure in the vicinity of a G-U pair . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 19.2.6 Structure of aminoacyl-tRNA and transacylation of the aminoacyl residue . . 19.3 Structure of elongation factor Tu . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 19.3.1 Sequence of Thermus thermophilus EF-Tu . . . . . . . . . . . . . . . . . . . . . . . . . . 19.3.2 Crystallization, X-ray analysis, and the tertiary structure . . . . . . . . . . . . . . . 19.3.3 Nucleotide binding and GTPase reaction . . . . . . . . . . . . . . . . . . . . . . . . . . 19.3.4 Mechanism of GTP induced conformational change of EF-Tu . . . . . . . . . . . 19.3.5 Aminoacyl-tRNA in complex with EF-Tu 7 GTP . . . . . . . . . . . . . . . . . . . . . 19.3.6 1H NMR of yeast Phe-tRNAPhe EF-Tu 7 GTP complex . . . . . . . . . . . . . . . . 19.3.7 13C NMR studies of the Val-tRNAVal EF-Tu 7 GTP ternary complex . . . . . . . 19.3.8 Role of EF-Tu in complex with aminoacyl-tRNA . . . . . . . . . . . . . . . . . . . . . 19.3.9 EF-Tu interaction with EF-Ts . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 19. 3. 10 Site-directed mutagenesis of EF-Tu . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 19.4 Summary and conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Acknowledgement . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
369
19
20 20.1 20.2 20.2.1
XII
Spectroscopic Probes of Surfactant Systems and Biopolymers . . . . . . Alexander Wokaun Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Diffusion in surfactant systems . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Structural characteristics of micellar solutions, cubic phases, and multilamellar vesicles from NMR self-diffusion measurements . . . . . . . . . . .
369 370 371 374 377 379 380 382 383 384 386 387 388 389 391 393 395 395 396 397 397 398
...
401
... ...
401 402
...
402
Contents 20.2.2 20.2.3 20.2.4 20.3 20.3.1 20.3.2 20.3.3 20.3.4 20.4 20.5
21 21.1 21.2 21.3 21.4 21.5 21.6 21.7
Probing of mobilities in multilamellar vesicles by forced Rayleigh scattering Dimensionality of diffusion in lyotropic mesophases from fluorescence quenching . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Summary of results . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Vibrational spectroscopy and conformational analysis of oligonucleotides . . Spectroscopic characterization of right and left-helical forms of a hexadecanucleotide duplex . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . SERS spectra of deoxyribonucleotides . . . . . . . . . . . . . . . . . . . . . . . . . . . . Studies of chromophore-DNA interaction by vibrational spectroscopy . . . . . Summary of results . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Related projects carried out within the framework of the Collaborative Research Centre . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Remarks and acknowledgements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
405
Energy Transport by Lattice Solitons in a-Helical Proteins . . . . . . . . Franz-Georg Mertens, Dieter Hochstrasser, and Helmut Büttner Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . The model . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Quasicontinuum approximation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Velocity range for the quasicontinuum approach . . . . . . . . . . . . . . . . . . Solitary waves for realistic parameter values . . . . . . . . . . . . . . . . . . . . . Iterative method and stability . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Conclusion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
...
424
... ... ... ... ... ... ... ...
424 426 428 431 432 434 437 438
...
443
... ... ... ...
443 444 444 444
... ... ... ... ... ...
445 446 447 450 457 459
IV
Appendix
22
Documentation of the Collaborative Research Centre 213 . . . . . . . . . Markus Schwoerer and Heinz Hoffmann List of Members . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Heads of Projects (Teilprojektleiter) . . . . . . . . . . . . . . . . . . . . . . . . . . . Projektbereich A: Gemeinsame Einrichtungen . . . . . . . . . . . . . . . . . . . Projektbereich B: Festkörper . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Projektbereich C: Funktionale Systeme – Mizellen, Oberflächen und Polymere . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Projektbereich D: Biopolymere . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Guests . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Co-workers . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . International Cooperation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Funding . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
22.1 22.2 22.2.1 22.2.2 22.2.3 22.2.4 22.3 22.4 22.5 22.6
409 412 413 413 415 417 418 419 421 422
XIII
Preface
At the end of 1983, about eight years after the inauguration of the University of Bayreuth the Deutsche Forschungsgemeinschaft (DFG) agreed to establish the Collaborative Research Centre 213, TOPOMAC, for the promotion of basic research in chemistry and physics of macromolecular systems. The title of TOPOMAC in its full length, “Topospezifische Chemie und Toposelektive Spektroskopie von Makromolekülsystemen: Mikroskopische Wechselwirkung und Makroskopische Funktion” expessed the intention of the original applicants: a productive cooperation between physicists, chemists and biochemists across the mutual borders of their original research fields. Until the end of 1995 TOPOMAC was supported by the Deutsche Forschungsgemeinschaft with 28 MDM. The present book documents the achievements of TOPOMAC. It is not a minute addition of all the results which have been published in periodical journals but rather a survey of important research fields of members of TOPOMAC. The articles have been written towards or after the end of the support period as both, review and original publications. The book covers the fields of: . Electronic, photoelectric, thermal, dielectric, optical and magnetic properties of macromolecular solids (polymers and polymer crystals), . Micellar structures, J-aggregates, liquid crystals, µ-gels, ferrocene-containing polymers and topospecific chemistry at surfaces and in single crystals, and . Biopolymers and surfactant systems as studied by site directed spectroscopy and site directed chemistry and also by the theory of energy transport. During the period of its support TOPOMAC had 30 members (Teilprojektleiter). Only ten of them have been members for the entire period, mainly because twenty times a call from other universities or research institutions reached one of the members of the Collaborative Research Centre 213. Fourteen of them followed this call and left the Collaborative Research Centre 213. Less than two years after the end of the period of support some of the remaining former members of Collaborative Research Centre 213 together with young and new faculty members began to continue the formal cooperation between chemists and physicists in the field of macromolecular research. Their actual cooperation in the meantime never had been terminated. The editors would like to express the sincere thanks of the members of TOPOMAC to the foreign guests of TOPOMAC, to the Deutsche Forschungsgemeinschaft, to the University XV
Preface of Bayreuth and also to the Freistaat Bayern. Our foreign guests stayed for long or short periods between one year and one day. They have contributed in an essential and special manner to the success on our research fields. They also strongly intensified the national and international scientific relations of both, the members and the research students of TOPOMAC. The cooperation of the speakers of TOPOMAC with Dr. Funk from the Deutsche Forschungsgemeinschaft office throughout the entire period of support was excellent. The help of the former president of the university, Dr. K. D. Wolff and his chancellor, W. P. Hentschel as well as the continuous support by the late Ministerialrat G. Grote and by J. Großkreutz from the Bayerisches Staatsministerium für Unterricht, Kultus, Wissenschaft und Kunst has been an essential stimulus for the scientific members of TOPOMAC. Last but not least we thank Doris Buntkowski for her faithful and reliable work as our secretary. The Editors
XVI
List of Contributors
Alexander Blumen Theoretische Polymerphysik Universität Freiburg Herrmann-Herder-Straße 3 79104 Freiburg
Dietrich Haarer Experimentalphysik IV Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Elmar Dormann Physikalisches Institut Universität Karlsruhe Engesserstr. 7 67131 Karlsruhe
Heinz Hoffmann Physikalische Chemie I Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Pablo Esquinazi Institut für Experimentelle Physik II Universität Leipzig Linnestraße 5 04103 Leipzig
Lorenz Kramer Theoretische Physik II Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Klaus Fesser Fachbereich Physik Universität Greifswald Domstraße 10 a 17489 Greifswald
Hans Ludwig Krauss Heunischstraße 5 b 96049 Bamberg
Josef Friedrich Lehrstuhl für Physik Technische Universität München 85350 Freising-Weihenstephan
Franz G. Mertens Theoretische Physik Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Holger Fehske Theoretische Physik I Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Oskar Nuyken Lehrstuhl für Makromolekulare Stoffe Technische Universität München Lichtenbergstraße 4 85747 München XVII
List of Contributors Sabine Rentsch Institut für Optik und Quantenelektronik Friedrich Schiller Universität Jena Max-Wien-Platz 1 07743 Jena
Alois Seilmeier Physikalisches Institut Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Wolfgang Richter Experimentalphysik IV Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Mathias Sprinzl Biochemie Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
Paul Rösch Biopolymere Universität Bayreuth Universitätsstraße 30 95447 Bayreuth Manfred Schmidt Institut für Physikalische Chemie Universität Mainz Welder-Weg 11 55099 Mainz Markus Schwoerer Experimentalphysik II Universität Bayreuth Universitätsstraße 30 95447 Bayreuth
XVIII
Peter Strohriegel Makromolekulare Chemie I Universität Bayreuth Universitätsstraße 30 95447 Bayreuth Thomas Vogtmann Experimentalphysik II Universität Bayreuth Universitätsstraße 30 95447 Bayreuth Alexander Wokaun Bereich F5 Paul Scherrer Institut CH-5232 Villingen
I
Mainly Solids
Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
1
Model Systems for Photoconductive Materials Harald Meyer and Dietrich Haarer
1.1
Introduction
The effect of photoconductivity, i. e. the increase of the electrical conductivity of a material upon illumination with light of suitable photon energy, was first discovered in selenium by W. Smith in 1873. A typical application for these materials is the xerographic process [2, 3], which was developed by C. F. Carlson in 1942 [1]. Here, a photoconducting film on top of a grounded electrode is homogeneously charged by a corona discharge. Typical field strengths are up to 106 V/m. In a second step the image of the original document is projected onto the film. At the areas where the film is illuminated charge carriers are generated in the photoconducting film. One species traverses the film and recombines at the grounded electrode whereas the oppositely charged species neutralizes the surface charges. With this step the original image is transferred into an electrostatic image on the photoconductor film. Subsequently, small toner particles are deposited on the photoconductor. They stick to the charged regions and thus generate a real image. In the next step, this image is transferred onto paper and fixed by thermally fusing the toner particles on the paper. The process for a laser printer is similar except for the fact that the image is written onto the photoconductor directly by a laser or a diode array. If the toner particles are fused directly onto the photoconductor instead of transferring them onto paper the photoconductor can be used as an offset printing master [4]. Potential systems for commercial use have to meet several requirements: a) sensitivity in the visible region of the spectrum; b) good charge transport properties, i. e. charge carrier mobility in excess of 10 –7 cm2/Vs [3] and minor trapping effects; c) good mechanical and dielectrical properties; d) excellent film forming properties and possibility of manufacturing defect free large area films; e) mechanical flexibility for the use in small sized desktop devices. The last two requirements cannot be met neither by organic nor inorganic crystalline materials. Therefore both, organic and inorganic amorphous photoconductors, have been deMacromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
3
1 Model Systems for Photoconductive Materials veloped. Inorganic materials like e. g. a-Se, As2Se3 or alloys of Se and Te show good transport properties with mobilities in the range of 0.1 cm2/Vs at room temperature [7], and high sensitivity for visible light together with moderate mechanical and dielectric properties. One of their most important disadvantages compared to organic systems is that most of these materials are highly toxic. In the past 30 years, since H. Hoegl discovered photoconductivity in the organic polymer poly(N-vinylcarbazole) (PVK) (Fig. 1.2) [5, 6], organic materials have almost completely replaced their inorganic counterparts, although the effective mobility in these systems is typically 5 orders of magnitude lower as compared to a-Se. Organic photoconductors can be regarded as large or medium bandgap semiconductors. A typical value for commercially applied systems is 3.5 eV for carbazole derivatives (Section 1.4). This inherent lack of sensitivity in the visible region has been overcome by using charge transfer systems [5] or multilayer systems with additional charge generation layers. For a review see e. g. Ref. [3]. On the other hand, the large bandgap of organic materials virtually eliminates the influence of thermally generated charge carriers and thus improves the dielectric properties as compared to low bandgap materials. Therefore the main target of the works, which will be described in the following, was to identify the key factors which limit the charge carrier mobilities in organic systems and to develop new high mobility materials.
1.2
Experimental techniques
Besides the xerographic discharge method [3, 10], the time-of-flight (TOF) technique is generally used to study the charge carrier transport of thin organic films. Here, the photoconducting film with a typical thickness of 10 mm is sandwiched between two electrodes (Fig. 1.1). Electron-hole pairs are generated by the energy hn of a strongly absorbed laser pulse, which is irradiated through one of the semitransparent electrodes. For most organic materials the charge carrier generation process can be described by an Onsager model, either in its one or three dimensional form [11–13]. The wavelength of the laser is chosen to ensure that the penetration depth is considerably less than the sample thickness. Thus the charge carriers are generated close to the illuminated surface. Under the influence of an externally applied electrical field the electronhole pairs are separated and one species, depending on the polarity of the external field, immediately recombines at the illuminated electrode. The opposite charged species drifts through the sample, thus giving rise to a time dependent photocurrent Ip (t). For a quantitative analysis the knowledge about the electrical field inside the sample is necessary. This can be achieved by performing the measurements in the small signal limit, i. e. disturbations due to space charge effects are negligible and the electric field in the bulk is determined by the externally applied field. It turns out, that this condition is fulfilled as long as the generated photocharge Qtot is less than 10 % of the charge Q = CU, which is 4
1.3
Transport models
Figure 1.1: Principle setup for TOF experiments.
stored on the electrodes. With typical experimental parameters (sample thickness d = 10 mm, sample area A = 4 cm2, 1021 monomer units per cm3, voltage U = 300 V, sample capacitance C = 1 nF) the above criterion leads to an upper limit for the photocharges of Qtot < 30 nF, corresponding to more than 26107 monomer units per charge carrier. For TOF experiments blocking contacts, e. g. Al for hole transport, have to be used to avoid trap filling due to an unduly large dark current. The quasi-Fermi energy e fp can be estimated from [69] p0 Nc exp
"f p =kB T; V
1
where V is the sample volume, p0 the number of charge carriers due to the dark current, and Nc is the density of states at the mobility edge. With typical values Nc = 1019 cm –3, T = 300 K, p0 = 36104 cm –3, equivalent to a dark current Id = 1 nA [68], the quasi-Fermi energy can be estimated to be approximately 0.83 eV. As will be shown later in Section 1.4, typical trap depths are of the order of 0.50 eV or less and therefore trap filling effects due to the dark current are not expected for the system under consideration.
1.3
Transport models
Basically two models are used to interpret the charge carrier transport properties of amorphous solids in the high temperature regime. The Multiple Trapping (MT) model [46] is based on the assumption that there exists a well-defined energy ed which separates electronic states where charge carriers are highly mobile from localized traps. In the conventional band picture this energy can be identified with the mobility edge. In the MT model the transport occurs by a sequence of trapping and detrapping events. Direct transfer between two traps is 5
1 Model Systems for Photoconductive Materials neglected, or in other words, the detrapping always occurs to states at ed . The traps can be caused by static disorder as well as by self trapping due to polaronic effects or both. Mathematically equivalent with the MT model is the Continuous Time Random Walk (CTRW) model [47–49], where the exponential trap distribution density g (e) in the MT model, " g
" / exp ;
2 kB T 0 corresponds to the well-known algebraic distribution of hopping times in the CTRW model [45],
t / t
1
;
3
where the disorder parameter a in Eq. 3 corresponds to the dimensionless temperature (a = T/T0). A variety of experimental data [16, 25, 26, 33, 34] can be described by the empirical formula, p "0 E ef f 0 exp ;
4 kB Tef f first proposed by Gill [33], where e0 is the zero field activation energy, E the electrical field and b the Poole-Frenkel factor. This equation describes the thermal activated release from localized traps where the activation energy is lowered by an external field according to the Poole-Frenkel effect [37]. The effective temperature Teff is related to the physical temperature T by 1 1 Tef f T
1 : T0
5
Initially, the characteristic temperature T0 simply was an empirical parameter. In Section 1.4, however, we shall see that in certain cases this parameter can be interpreted microscopically. An alternative approach [28, 50–54] is based on the assumption that the density of states can be modelled by a Gaussian distribution. Charge carrier transport occurs via direct hopping between the localized sites. In general, the differences between the two models are too small to be detected experimentally. Since our data can be quantitatively explained within the framework of multiple trapping we will restrict the discussion to this model.
6
1.4
1.4
Results
Results
As stated in Section 1.1, organic photoconductors can be regarded as large or medium bandgap semiconductors. In contrast to inorganic crystalline semiconductors the electronic coupling between adjacent sites is weak. Therefore the electronic states in these materials are primarily of molecular character and the charge carrier transport has to be regarded as an incoherent hopping process between two neighbouring sites. For the following discussion organic photoconductors will be divided into three main groups namely molecularly doped polymers (Section 1.4.1), side-chain polymers (Section 1.4.2.), and conjugated systems (Section 1.4.3).
1.4.1 Molecularly doped polymers In molecularly doped polymers (MDPs) the transport molecules are molecularly dispersed in an inert matrix. Due to crystallization the maximum concentration of chromophores, which can be achieved, is typically in the range of 50 mol%. Typical chemical compounds include oxadiazole derivatives [14], pyrazolines [15– 18], hydrazones [19–22], carbazole derivatives [23–26], triphenylmethane (TPM) derivatives [27, 28], triphenylamine (TPA) derivatives [29, 30], and TAPC [31], which can be regarded as a dimer of TPA. The charge carrier mobilities at room temperature are typically in the range from 10 –6 cm2/Vs for N-isopropylcarbazole [25] to 10–4 cm2/Vs for p-diethylaminobenzaldehyde diphenyl hydrazone (DEH) [22]. In order to study the effect of chemical substitutions of the respective transport molecule N-isopropylcarbazole (NIPC) and derivatives thereof, with electron donor as well as acceptor substituents (Fig. 1.2), have been investigated in a polycarbonate host [26]. As compared by 3,6-dibromo-N-isopropylcarbazole (DBr-NIPC) the effective hole mobility of 3,6-dimethoxy-N-isopropylcarbazole (DMO-NIPC) is slightly decreased. The reason for this behaviour is the fact that the cation, which is relevant for the transport process, is stabilized by electron donating substituents like the methoxy group, as can be seen from the shift of the ionisation potentials [26]. This leads to stronger localization of the charge within the aromatic rings as compared to derivatives with moderate electron acceptors like bromine. Therefore the spatial overlap of the electronic states of adjacent molecules, which are involved in the transport process, is reduced. With strong acceptors like the nitro groups in 3,6-dinitro-N-isopropylcarbazole (DNNIPC) the ionisation potential is already larger than for the host matrix polycarbonate. In this case even the matrix acts as a trap for holes, thus preventing efficient charge carrier transport [26]. Since the effective mobility is determined by the spatial overlap of the transport states, the concentration dependence of the effective mobility can be described by ef f / r2 exp
2r ; r0
6
7
1 Model Systems for Photoconductive Materials
H3CO
N
R
N N
C2H5 N BTA
R
R:
H: Br: OCH3: NO 2:
N
NIPC DBr-NIPC DMO-NIPC DN-NIPC
Si CH3 CH
Si
CH2
Ca
O
n
PMPS
(CH2)n
n
PVK
Ca
R
n
Polysiloxan
R N Ca:
R:
n
O DPOP-PPV H
PPV
Figure 1.2: Chemical structure of photoconducting materials. Abbreviations see text.
where r is the mean distance between adjacent transport molecules and r0 the wave function decay parameter. For carbazole derivatives r0 is typically in the range 1.3–1.6 Å, depending on the substituted groups [26]. In recent years, also percolation models have been successfully applied to experimental data [55] as an alternative approach to model the transport properties of doped disordered systems. For polycarbonate doped with a derivative of benztriazole (BTA) (Fig. 1.2) it has been shown that the concentration dependence of the effective mobility can be described at low concentrations by [55] ef f 0
p
pc t
7
for p > pc , where p is the concentration of transport molecules, pc the percolation threshold, and t the critical exponent. The experimental values (pc = 0.095 and t = 2.46) are consistent with 3D-continuum percolation calculations [56]. Since this system shows good transport properties over a wide range of concentrations, the influence of extrinsic traps could be studied [57]. Here, a sample containing 25 wt% of BTA in a polycarbonate host was doped with small amounts of the organic dye astrazone orange (AO). It turned out that the effective mobility is reduced by a factor of 2 when the 8
1.4
Results
concentration of AO is increased to 0.5 wt%. This finding becomes also important when thinking of new applications like organic electroluminescent devices. One way to increase the efficiency in these devices is to molecularly disperse the luminescent moiety into a charge transport material. But there is a trade-off between efficient trapping of the charge carriers – which is improved by higher concentrations of the luminescent groups – and concentration quenching of the fluorescence, which can be avoided by keeping the concentration as low as possible. The above described measurements [57] show that organic dyes can be very efficient traps for charge carriers. Therefore the concentration of the luminescent moiety can be as low as 2 % or less [61], thus avoiding concentration quenching without loosing high trapping efficiency.
1.4.2 Side-chain polymers In side-chain polymers, where the chromophore is covalently bonded to a polymer main chain, the concentration of transport molecules can be increased as compared to MDPs without causing crystallization. Because the underlying physical mechanism of charge carrier transport (nearest neighbour hopping between weakly coupled, localized states) is the same for both MDPs and side-chain polymers, the transport properties are qualitatively similar. This finding offers the opportunity to tailor the thermal and mechanical properties of the photoconductor without seriously affecting the transport properties. This can be achieved either by variation of the spacer length between the chromophore and the backbone or by variation of the backbone itself. A typical example for this group is PVK [12, 32, 34, 35]. Here, the transition from dispersive to non-dispersive transport could be observed [34]. Due to the fact, that the TOF curves have been measured over 10 decades in time, it was possible by means of a numerical inverse Laplace transform [34] to calculate from the measured photocurrent the trapping rate distribution, which is a measure for the density of localized states. In polysiloxane derivatives with pendant carbazolyl groups [58, 59] (Fig. 1.2) the effect of a variation of the spacer length was investigated. Starting from a spacer length of 3 or 5 methylene units up to 6 or 11 groups, the glass transition temperature drops from its initial value of 51 8C or 7 8C down to –5 8C or – 45 8C for the C11 spacer. It turns out, that the zero field activation energy eact for the hole transport remains unchanged and is the same for NIPC or PVK, eact = 0.51 eV [58]. This indicates, that the activation energy in side-chain polymers with pendant carbazolyl groups is dominated by intrinsic properties of the carbazolyl moiety and is not much affected by other factors like the morphology of the polymer [58]. However, the absolute values for meff differ by roughly one order of magnitude, where the compound with the shortest spacer shows an effective mobility in the range of 10 –6 cm2/Vs (T = 300 K, E = 3 7 105 V/cm). For the materials with a spacer length of 5 and 6 methylene units the mobility is lower by one order of magnitude and therefore comparable to the mobility in NIPC or PVK. A striking feature, when comparing NIPC with PVK, is the fact that polycarbonate doped with 20 wt% of NIPC shows the same hole mobility at room temperature as compared to PVK where the carbazole concentration amounts to 86 wt%. Obviously, the covalent attachment of the chromophore to a stiff backbone, like PVK with its glass transition temperature of 227 8C, induces a mutual orientation of adjacent pendant groups, 9
1 Model Systems for Photoconductive Materials which reduces the electronic coupling between the two sites. Therefore it is desirable to induce a well-defined amount of flexibility in both, the spacer and the backbone, to allow for mutual reorientation of the chromophores. For a polysiloxane backbone with carbazolyl transport groups the optimum spacer length n is equal to 3.
1.4.3 Conjugated systems In contrast to the two main groups described above the charge carrier transport in conjugated systems occurs via the polymer backbone. Various substituents are used to tailor the mechanical properties and the processibility. For instance, the chain can be a skeleton with quasi-s-conjugation like in polysilanes [36, 38–42] or polygermylenes [39]. The second group of main chain polymers contains a p-conjugated backbone like polyacetylene, polythiophene, polypyrrole, polyphenylene, poly(phenylenevinylene) (PPV), and their derivatives. For a review see [43, 44]. Both types of conjugated systems have been investigated. In the case of poly(methylphenyl silane) (PMPS), a quasi-s-conjugated polymer (Fig. 1.2), non-dispersive transport has been found down to a temperature of 250 K [60]. For lower temperatures, the transport is dispersive, which indicates that the transport in these materials is controlled by traps. Compared to the materials described above, the depths of the relevant traps are much lower. The zero field activation energy turns out to be as low as 0.37 eV as compared to 0.5 eV for materials containing carbazole. This gives a hole mobility at room temperature of roughly 10 –3 cm2/Vs, which is 3 orders of magnitude higher than for the materials described above. The high mobility and the transparency in the visible region makes PMPS also useful for applications in multilayer electroluminescent devices [61–63]. Besides the s-bonded PMPS, we investigated oligomeric conjugated compounds based on carbazole [64]. First experiments with a trimer of a carbazole derivative showed that this material is soluble in most of the common organic solvents. It forms a low molecular weight glass and shows no tendency to crystallize even after several months. In this material the p-system has been extended over three monomer units, which results in remarkably high hole mobilities as compared to the monomer model compound NIPC. First TOF experiments show an increase in mobility by roughly two orders of magnitude as compared to unconjugated carbazole systems, which reaches 2 7 10 –4 cm2/Vs [64]. The second group of p-conjugated polymers contains one pz-orbital per carbon atom which stands perpendicular to the plane of the s-bonded skeleton of the main chain. The interaction between these orbitals leads to electronic states, which are delocalized – at least partly – along the conjugated chain. As compared to the intrachain coupling, the intrachain coupling is lower by typically one or two orders of magnitude [66] thus leading to a large anisotropy of the electronic and optical properties. These materials can be regarded as basically one-dimensional organic semiconductors with bandgaps in the visible region of the spectrum, e. g. 1.5 eV (trans-(CH)x) [43], 2.0 eV (polythiophene), 2.5 eV (polyphenylene vinylene), and 3.0 eV [poly(para-phenylene)] [67]. We investigated the charge transport properties of the p-conjugated polymer poly (para-phenylenevinylene) and its soluble substituted derivative DPOP-PPV (Fig. 1.2). In 10
1.4
Results
contrast to e. g. (CH)x , PPV can be prepared in undoped form. If oxygen is carefully heated out, PPV exhibits excellent film forming properties as well as thermal stability under ambient conditions. In recent years, PPV has drawn additional attention due to its use in organic electroluminescent devices [45]. In the following we will show that the charge carrier transport in these materials can be described by the conventional models mentioned before, which have been developed for the characterization of disordered molecular systems. Based on the MT model a method has been developed to calculate the distribution of capture rates from the measured photocurrent [68, 69]. In contrast to Ref. [34], the method is based on a Fourier transform technique with better numerical stability as compared to the inverse Laplace transform used in Ref. [34]. With this approach the capture rate density oc is given by 2 !c
"! kB T p
Qtot sin tmic I
!
! ! ;
8
where Qtot is the total photogenerated charge, tmic the microscopic transit time, and I (o) the Fourier transform of the measured photocurrent, and f the phase shift (Eq. 9). For DPOPPPV, tmic = 7.5610–10 s for the given experimental conditions. tan
1
Im I
! Re I
!
9
The trap depth eo is related to the frequency o by the expression ! r0 exp
"! ; kB T
10
where r0 is the attempt-to-escape frequency (r0 = 1010 s –1 for DPOP-PPV). In DPOP-PPV the effective mobility is field dependent and thermally activated according to Gill’s formula (Eq. 4) [33] with a characteristic temperature T0 = 465 K (Fig. 1.3). The calculated trap density g (e) is exponential down to a pronounced cutoff energy ed , g
" / exp
" : kB T 0
11
This cutoff energy corresponds exactly to the measured activation energy of the effective mobility. Furthermore, the initially simply empirical parameter T0 in Gill’s formula (Eq. 4) could be correlated with the decay constant kBT0 of the trap distribution. By calculating the total number of trapping events it can be seen that the typical distance which a charge carrier travels between two trapping events is of the order of 4 Å. This value is comparable to the intrachain distance and indicates that the transport in these materials can be best described by conventional hopping between closely neighbouring sites. No evidence for bandlike transport has been found. 11
1 Model Systems for Photoconductive Materials 350 K
-2
10
300 K
500 kV/cm 350 kV/cm 200 kV/cm 75 kV/cm 0 kV/cm
-3
10
-4
10 2
µeff [cm /Vs]
230 K
270 K
-5
10
2
10
0
T0 = 465K
10
-6
10
-2
10
-4
10
-6
10
-7
-8
10
10
-10
10
0
2
4
6
8
-8
10
2.5
3.0
3.5 1/T [1000/K]
4.0
4.5
Figure 1.3: large frame: effective mobility meff of DPOP-PPV as a function of temperature for some electrical fields, data points for zero field were extrapolated from field dependent measurements; inset: Arrhenius fits for different electrical fields. For details see text. Data from [68, 69].
For the case of PPV the dispersion of the photocurrent is too large for transit time determination. It can be concluded that even at room temperature the release times from the deepest traps, which control the transport properties, are in the range of 1 s or less. This corresponds to an effective mobility of less than 10–8 cm2/Vs [69]. Based on TSC measurements from different groups [70], we conclude that this behaviour is primarily caused by the existence of grain boundaries. It is reasonable to assume that in conjugated polymers with a rigid backbone the preferred orientation of the main chain will be parallel to the film surface. Therefore, the charge carrier transport through the film has to occur perpendicular to the backbone, i. e. perpendicular to the direction with high intrinsic mobility, which would mean a principle limit for this class of materials for this kind of applications.
1.5
Outlook
As described above, disordered organic materials have been developed with effective hole mobilities of up to 10–3 cm2/Vs together with good mechanical and dielectric properties. However it seems that for disordered systems a considerable improvement of this value will 12
References be difficult to achieve, because for all investigated material groups the charge carrier transport is limited by the localized nature of the electronic states and by the hopping mechanism of the transport process. Based on recent other works [8, 9], we think that for developing even higher mobility materials it is essential to improve the structural order of the material. This may open new application fields, e. g. the use of active organic materials in semiconductor devices. One promising way is the use of highly ordered liquid crystals. With these materials, however, charge carrier mobilities up to 0.1 cm2/Vs or even more are realistic, which would make them comparable to single crystalline systems [65].
References
1. 2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29.
C. F. Carlson: US Pat. 2 297 691 (1942) D. Haarer: Angew. Makromol. Chem., 183, 197 (1990) D.M. Pai, B.E. Springett: Rev. Mod. Phys., 65(1), 163 (1993) K.-W. Klüpfel, M. Tomanck, F. Endermann: German Patent No. DE-B-11 45 184 (1963) H. Hoegl, O. Süs, W. Neugebauer, Kalle AG: German Patent No. DBP 1068115. Chem. Abstr., 55, 20742 a (1961) H. Hoegl: J. Phys. Chem., 69(3), 755 (1965) G. Pfister: Phys. Rev. Lett., 36(5), 271 (1976) D. Adam, F. Closs, T. Frey, D. Funhoff, D. Haarer, H. Ringsdorf, P. Schuhmacher, K. Siemensmeyer: Phys. Rev. Lett., 70(4), 457 (1993) D. Adam, P. Schuhmacher, J. Simmerer, L. Häussling, K. Siemensmeyer, K.H. Etzbach, H. Ringsdorf, D. Haarer: Nature, 371, 141 (1994) H. Tung Li, P.J. Regensburger: J. Appl. Phys., 34, 1730 (1963) L. Onsager: Phys. Rev. B, 54, 554 (1938) H. Kaul, D. Haarer: Ber. Bunsenges. Phys. Chem., 91, 845 (1987) M. Gailberger, H. Bässler: Phys. Rev. B, 44(16), 8643 (1991) Y. Kanemitsu, Y. Sugimoto: Phys. Rev. B, 16(21), 14 182 (1992) Y. Sano, K. Kato, M. Yokoyama, Y. Shirota: H. Mikawa, Mol. Cryst. Liq. Cryst. 36(1–2), 137 (1976) A. Peled, L.B. Schein, D. Glatz: Phys. Rev. B, 41(15), 10 835 (1990) Y. Kanemitsu, H. Funada, Y. Masumoto: J. Appl. Phys., 71(1), 300 (1992) H. Bässler, P.M. Borsenberger: Chem. Phys., 177(3), 763 (1993) P.N. Sanda, T. Takamori, D.B. Dove: J. Appl. Phys., 64(3), 1229 (1988) J.X. Mack, L.B. Schein, A. Peled: Phys. Rev. B, 39, 7500 (1989) Y. Kanemitsu, H. Funada, S. Imamura: J. Appl. Phys., 67(9), 4152 (1990) P.M. Borsenberger, L.T. Pautmeier, H. Bässler: Phys. Rev. B, 46(19), 12 145 (1992) J. Mort, G. Pfister, S. Grammatica: Solid State Commun., 18, 693 (1976) P.M. Borsenberger, L.E. Contois, A.I. Ateya: J. Appl. Phys., 50(2), 914 (1979) S.J. Santos Lemus, J. Hirsch: Philos. Mag. B, 53(1), 25 (1986) D. Haarer, H. Meyer, P. Strohriegl, D. Naegele: Makromol. Chem., 192(3), 617 (1991) D.M. Pai, J.F. Yanus, M. Stolka, D. Renfer, W.W. Limburg: Philos. Mag., 48(6), 505 (1983) H. Bässler: Philos. Mag., 50(3), 347 (1984) G. Pfister: Phys. Rev. B, 16(8), 3676 (1977)
13
1 Model Systems for Photoconductive Materials 30. P.M. Borsenberger: J. Appl. Phys., 68(12), 6263 (1990) 31. P.M. Borsenberger L. Pautmeier, R. Richert, H. Bässler: J. Chem. Phys., 94(12), 8276 (1991) 32. J.M. Pearson, M. Stolka: Polymer Monographs, Vol. 6: Poly(N-vinylcarbazole), Gordon and Breach Sci. Publ., New York (1981) 33. W.D. Gill: J. Appl. Phys., 43, 5033 (1972) 34. E. Müller-Horsche, D. Haarer, H. Scher: Phys. Rev. B, 35, 1273 (1987) 35. F.C. Bos, D.M. Burland: Phys. Rev. Lett., 58, 152 (1987) 36. R.G. Kepler, J.M. Zeigler, L.A. Harrah, S.R. Kurtz: Phys. Rev. B, 35(6), 2818 (1987) 37. J. Frenekl: Phys. Rev., 54, 647 (1938) 38. K. Shimakawa, T. Okada, O. Imagawa: J. Non-Cryst. Solids, 114(1), 345 (1989) 39. M. Abkowitz, M. Stolka: Solid State Commun., 78(4), 269 (1991) 40. H. Kaul: PhD thesis, Universität Bayreuth (1991) 41. E. Brynda, S. Nespurek, W. Schnabel: Chem. Phys., 175(2–3), 459 (1993) 42. V. Cimrova, S. Nespurek, R. Kuzel, W. Schnabel: Synth. Met., 67(1–3), 103 (1994) 43. A.J. Heeger, S. Kivelson, J.R. Schrieffer, W.-P. Su: Rev. Mod. Phys., 60(3), 781 (1988) 44. J. L. Brédas, R. Silbey (eds.): Conjugated Polymers, Kluwer Academic Publishers, Dordrecht (1991) 45. J.H. Burroughes, D.D.C. Bradley, A.R. Brown, R.N. Marks, K. Mackay, R.H. Friend, P.L. Burns, A.B. Holmes: Nature, 347(6293), 539 (1990) 46. F.W. Schmidlin: Phys. Rev. B, 16(6), 2362 (1977) 47. H. Scher, E.W. Montroll: Phys. Rev. B, 12(6), 2455 (1975) 48. J. Noolandi: Phys. Rev. B, 16(10), 4474 (1977) 49. G. Pfister, H. Scher, Adv. in Phys, 27(5), 747 (1978) 50. P.M. Borsenberger, L. Pautmeier, H. Bässler: J. Chem. Phys., 94(8), 5447 (1991) 51. G. Schönherr, H. Bässler, M. Silver: Philos. Mag. B, 44(3), 369 (1981) 52. H. Bässler, G. Schönherr, M. Abkowitz, D.M. Pai: Phys. Rev. B, 26(6), 3105 (1982) 53. L. Pautmeier, R. Richert, H. Bässler: Philos. Mag. Lett., 59(6), 325 (1989) 54. L. Pautmeier, R. Richert, H. Bässler: Synth. Met., 37, 271 (1990) 55. H. Domes, R. Leyrer, D. Haarer, A. Blumen: Phys. Rev. B, 36(8), 4522 (1987) 56. D. Stauffer: Introduction to Percolation Theory, Taylor and Francis, London (1985) 57. H. Domes: PhD thesis, Universität Bayreuth (1988) 58. H. Domes, R. Fischer, D. Haarer, R. Strohriegl: Makromol. Chem., 190, 165 (1989) 59. H. Schnörer, H. Domes, A. Blumen, D. Haarer: Philos. Mag. Lett., 58(2), 101 (1988) 60. H. Kaul: PhD thesis, Universität Bayreuth (1991) 61. H. Suzuki, H. Meyer, J. Simmerer, J. Yang, D. Haarer: Adv. Mater., 5, 743 (1993) 62. H. Suzuki, H. Meyer, S. Hoshino, D. Haarer: J. Appl. Phys. in press (1995) 63. J. Kido, K. Nagai, Y. Okamoto, T. Skotheim: Appl. Phys. Lett., 59, 2760 (1991) 64. C. Beginn, J.V. Grazulevicius, P. Strohriegl,J. Simmerer, D. Haarer: Macromol. Chem. Phys., 195, 2353 (1994) 65. N. Karl: in: K. Sumino (ed.): Defect Control in Semiconductors, Elsevier Science Publishers, North Holland (1990) 66. P. Gomes da Costa, R.G. Dandrea, E.M. Conwell: Phys. Rev. B, 47(4), 1800 (1993) 67. G. Leising, K. Pichler, F. Stelzer: in: H. Kuzmany, M. Mehring, S. Roth, (eds.): Springer Series in Solid-State Sciences, Vol. 91: Electronic Properties of Conjugated Polymers III, Springer, Berlin (1989) 68. H. Meyer: PhD thesis, Universität Bayreuth (1994) 69. H. Meyer, D. Haarer, H. Naarmann, H.H. Hörhold: Phys. Rev. B, in press (1995) 70. M. Onoda, D.H. Park, K. Yoshino: J. Phys. (London), Condens. Matter, 1(1), 113 (1989)
14
2 Novel Photoconductive Polymers Jörg Bettenhausen and Peter Strohriegl
2.1
Introduction
Electrophotography is the only area in which the conductivity of sophisticated organic materials and polymers is exploited in a large scale industrial process today. Photoconductors are characterized by an increase of electrical conductivity upon irradiation. According to this definition photoconductive materials are insulators in the dark and become semiconductors if illuminated. In contrast to electrically conductive compounds photoconductors do not contain free carriers of charge. In photoconductors these carriers are generated by the action of light. The discovery of photoconductivity dates back to 1873 when W. Smith found the effect in selenium. Based on this discovery C. F. Carlson developed the principles of the xerographic process already in 1938. Photoconductivity in organic polymers was first discovered in 1957 by H. Hoegl, who found that poly(N-vinylcarbazole) (PVK) and charge transfer complexes of PVK with electron acceptors like 2,4,7-trinitrofluorenone act as photoconductors [1]. Besides the application of photoconductive polymers in photocopiers these materials are also widely used in laser printers in the last years. The third area in which photoconductors are applied is the manufacturing of electrophotographic printing plates. The organic photoconductors used in practice are based on two types of systems. The first one are polymers in which the photoconductive moiety is part of the polymer, for example a pendant or in-chain group. The second group involves low molecular weight compounds imbedded in a polymer matrix. These so-called moleculary doped polymers are widely used today. One interesting class of photoconductive materials are oxadiazoles. It is known for a long time that derivatives of 1,3,4-oxadiazole are good photoconductors. Compound 1 for example is described in patents and was frequently applied in photocopiers [2].
1
2
Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
15
2
Novel Photoconductive Polymers
The oxadiazole 1 is a hole transport material since the electron withdrawing effect of the oxadiazole group with three electronegative heteroatoms is overcompensated by two electron donating amino groups. Within the last years, oxadiazoles like 2-(biphenyl)-5-(4-tert.butylphenyl)-1,3,4oxadiazole (PBD) 2 have been frequently applied in organic light emitting diodes [3]. Here the electron withdrawing oxadiazole unit dominates the electronic properties and the oxadiazole compounds act as electron injection and transport layers. Furthermore, 2,5-diphenyloxadiazoles have been used as building blocks in thermostable polymers and they are highly fluorescent as well. In this paper the synthesis and characterization of a number of novel low molecular weight oxadiazole derivatives and polymers is described. The compounds show different molecular shapes, e. g. rod-like and star-shaped structures have been realized. In addition to the compounds described here, a series of different main chain and side group polymers with oxadiazole moieties are presently synthesized in our research group [4].
2.2
Liquid crystalline oxadiazoles and thiadiazoles
2.2.1 The basic idea The aim of this work is the preparation of photoconductive compounds with high carrier mobilities. There are a number of indications that the carrier mobility, i. e. the speed of the charge particles within the sample, depends on the geometric arrangement of the photoconductive moieties. At room temperature for instance, the mobility in single crystals of aromatic compounds like anthracene or perylene is very high, i. e. in the range of 10–1 cm2/Vs [5]. In amorphous polymers the carrier mobilities are orders of magnitude smaller and typical values are in the range of 10–6 and 10 –8 cm2/Vs [6]. So we were interested to investigate if the higher order in the liquid crystalline state leads to higher mobilities in comparison to less ordered amorphous solids. In liquid crystalline polymers a macroscopic orientation of the photoconductive groups in the mesophase can be achieved by means of electric or magnetic fields. The orientation can be frozen in by lowering the temperature below the glass transition. By this, materials with a degree of order between a perfect single crystal and totally disordered amorphous polymers are obtained. With this in mind we started the synthesis of a series of liquid crystalline model compounds and polymers in which the side groups possess both mesogenic and photoconductive properties.
16
2.2
Liquid crystalline oxadiazoles and thiadiazoles
2.2.2 Monomer synthesis In the past years we have synthesized a variety of compounds with oxadiazole and thiadiazole moieties [7]:
3X=S
4X=O
The rod-like thiadiazole derivative 3 is liquid crystalline and shows a smectic as well as a nematic LC phase with the following phase behaviour: c 103 sa 180 n 203 i. An acrylate monomer was prepared by hydroboration of the terminal double bond and subsequent esterification with acryloyl chloride and then polymerized. The resulting polymer 5 exhibits a mesophase which has not yet been identified.
5
Unfortunately the clearing point of the polymer is at 246 8C, where the material starts to decompose. Therefore orientation in an electric field was not possible. In contrast to the thiadiazole the oxadiazole 4 is neither liquid crystalline as monomer nor as polymer. The reason for the lack of mesogenic properties is that the substitution of the sulphur by oxygen introduces a bend into the molecule which prevents the formation of a LC phase. Recently liquid crystalline oxadiazoles (Scheme 2.1) have been described [8]. Here the oxadiazole is coupled to at least two benzene or cyclohexane rings. Thereby an increase of the mesophase stability is achieved.
Scheme 2.1: Liquid crystalline oxadiazole compounds [8].
17
2
Novel Photoconductive Polymers
6
7
8
9
10-13
10
R = Ph-OC6H13
12
R = Ph-N(CH3)2
11
R = C7H15
13
R = Ph-N(CH3)C6H13
Scheme 2.2: Monomer synthesis.
Our aim was to synthesize a series of different oxadiazole monomers which are functionalized for the preparation of polymers. Scheme 2.2 shows the synthesis of the monomeric 1,3,4-oxadiazoles. The oxadiazole moiety is formed by a cyclisation reaction of the diacylhydrazine derivatives 8 with phosphorous oxychloride. The unsymmetrical bishydrazides 8 are prepared by treatment of benzoyl chlorides 6 with the appropriate monohydrazides 7. The last reaction step is an esterification with 4-(5-hexenyloxy)benzoyl chloride. The esterification reaction is essential in this case because of two reasons. First the rod-like 18
2.2
Liquid crystalline oxadiazoles and thiadiazoles
mesogen is formed, and second a functional group for the preparation of LC polymers is introduced. Additionally the oxadiazole monomer 14 was synthesized, in which the ester group is replaced by a biphenyl unit. By this it is possible to investigate the influence of the ester function on the photoconductive properties of the liquid crystalline compounds.
14
The liquid crystalline behaviour and the phase transitions of the monomeric oxadiazole derivatives 10–14 were determined by DSC and polarizing microscopy. In Tab. 2.1 the phase transition temperatures are summarized: Table 2.1: Phase behaviour of the monomeric oxadiazoles 10–14 Transition temperature in 8C
Compound 10 11 12 13 14
k k k k k
141 90 162 127 72
n sa n (sa sa
167 116 179 111) 77
i i i i i
Except compound 13 all monomers are enantiotropic liquid crystalline and show nematic or smectic mesophases. Only derivative 13 shows a monotropic sa phase.
2.2.3 Oligo and polysiloxanes with pendant oxadiazole groups The next step was the synthesis of liquid crystalline polysiloxanes with oxadiazole groups in the mesogenic unit. The polymers were prepared by a polymeranalogous reaction of the monomers 10 and 11 with poly(hydrogenmethylsiloxane) 15. Both polymers are liquid crystalline. The transition into the isotropic phase takes place at about 200 8C and therefore at a much higher temperature than in the monomers. The high clearing temperature makes the orientation of the polymers difficult which is preferably carried out near the clearing point. Up to now it was not possible to prepare well-defined polymers with the monomers 12–14. A possible reason is the inactivation of the Pt catalyst by the amino groups. If the cyclic tetrasiloxane 18, which is commercially available in high purity, is used instead of 15, well-defined monodisperse model compounds are obtained [9]. These com19
2
Novel Photoconductive Polymers
10, 11
16
R = Ph-OC6H13
15
17
R = C7H15
Scheme 2.3: Synthesis of polysiloxanes with pendant oxadiazole groups.
pounds can be highly purified, for example by preparative gel permeation chromatography. This is very important for photoconductors, because it is well-known that even traces of impurities may reduce the carrier mobility.
18
So the monomeric compounds 10 and 12–14 have been reacted with 18 to yield the following tetrameric derivatives:
19
R = Ph-OC6H13 , n = 1
21
R = Ph-N(CH3)C6H13 , n =
20
R = Ph-N(CH3)2 , n = 1
22
R = Ph-N(CH3)C6H13 , n =
Scheme 2.4: Tetrasiloxanes with pendant oxadiazole groups.
20
2.2
Liquid crystalline oxadiazoles and thiadiazoles
All cyclosiloxanes are liquid crystalline and show several advantages compared to the polymers. So the cyclic siloxanes form stable glasses but their clearing points are much lower. For example compounds 21 and 22 possess clearing temperatures at only 102 8C. The phase behaviour of the tetramers are listed in Tab. 2.2. Table 2.2: Phase behaviour of the tetrameric siloxanes 19–22. Transition temperature in 8C
Comp. 19 20 21 22
g g g g
54 67 34 38
m1 a) sa k sa
108 138 66 82
m2 a) n n n
117 181 102 102
sc i i i
155
n
185
i
a) Mesophase not identified
2.2.4 Photoconductivity measurements For the characterization of the novel photoconductive compounds two different experimental techniques have been used. Some measurements were made by BASF AG using a steady-state method. These experiments allow a quick characterization, but in contrast to the time-of-flight (TOF) method no statements about transient photocurrents and carrier mobilities are possible. The TOF measurements were carried out in the group of D. Haarer, Universität Bayreuth. The tetrameric cyclosiloxanes are very suitable compounds for physical investigations. Because of the low viscosity the preparation of samples is much easier than in the case of the polymers. Additionally the dark currents of the tetramers are very low. All the compounds are photoconductive, as shown by the steady-state method. For example, the measurements of the thiadiazole 3 showed a distinct rise of the photocurrent at the transition from the crystalline to the mesophase, as shown in Fig. 2.1. The decrease of
Figure 2.1: Temperature dependence of the photocurrent of the thiadiazole 3.
21
2
Novel Photoconductive Polymers
the current at the transition from the smectic to the nematic phase is directly correlated with the loss of order. These results show that the basic idea of this work is correct. Nevertheless, we were not able to carry out TOF measurements with calamitic monomers, because the dark currents in the liquid crystalline phases were too high. As mentioned before, such measurements are possible with the cyclic tetramers. The transient photocurrents of the tetrasiloxanes 19, 21, 22 illustrate that the carrier transport is totally dispersive, i. e. dominated by deep traps in which the charge carriers are captured. This is a typical behaviour of amorphous polymers. No transit time could be detected and no statements about the carrier mobility can be made for the rod-like mesogens. In contrast it was shown in the past years that discotic liquid crystals like hexapentyloxytriphenylene (HPT) 23 have carrier mobilities up to 10 –3 cm2/Vs in the liquid crystalline Dho phase [10]. Here, the disc-shaped molecules are ideally stacked above each other and therewith allow a fast carrier transport. The discotic hexathioether 24 with a highly ordered helical columnar (H) phase exhibits mobilities up to 10–1 cm2/Vs, which are almost as high as in organic single crystals [11].
6
6
23
24
One important observation during the photoconductivity measurements of the tetramer 19 was, that it showed almost the same photocurrent for holes and electrons. This was interesting because of the lack of electron transporting materials and led us synthesize a variety of starburst oxadiazole compounds, which are described in the next Chapter.
2.3
Starburst oxadiazole compounds
2.3.1 Motivation The synthesis of novel materials with high carrier mobilities is one of the major goals in the field of photoconductive polymers. Within the last years different approaches have been pursued to reach this goal. First, the photoconductive properties of conjugated polymers like poly(phenylenevinylene) and poly(methyl phenylsilane) have been investigated [12]. Another approach are liquid crystals which are the topic of the first Chapter. The third way to realize 22
2.3
Starburst oxadiazole compounds
the goal are glasses of large extended aromatic amines. The best investigated representatives of this class of compounds are N,N'-diphenyl-N,N'-bis(3-methylphenyl)-[1,1'-biphenyl]-4,4'diamine (TPD) 25 from Xerox [13] and 1,1-bis(di-4-tolyl-aminophenyl)cyclohexane (TAPC) 26 from Kodak [14]. Both compounds are derivatives of triphenylamine, a well-known photoconductor. If thin films of TPD and TAPC are prepared by vacuum evaporation both compounds form metastable glasses. In such glasses carrier mobilities up to 10–3 cm2/Vs for TPD [13] and 10 –2 cm2/Vs for TAPC [14] have been reported. But both TAPC and TPD glasses are metastable and have a strong tendency to crystallize. If the molecules are imbedded in a polymer matrix, e. g. polycarbonate or polystyrene, morphologically stable materials are formed, but the mobilities decrease drastically [13].
25
26
Several attempts have been made to overcome the problems with metastable TPD and TAPC glasses. Recently we described the synthesis of 3,6-bis[(9-hexyl-3-carbazolyl)ethynyl]-9-hexylcarbazole 27, a trimeric model compound of poly(carbazolylene ethynylene) [15]. This material shows a glass transition temperature of 41 8C and forms glasses which are stable for more than a year. Mobilities up to 10–4 cm2/Vs (E = 6 7 105 V/cm, T = 30 8C) have been measured by the time-of-flight technique.
27
Another interesting approach are starburst compounds with high glass transition temperatures. So 4,4',4@-tris(N-carbazolyl)triphenylamine, which has been published recently [16], shows a glass transition at 151 8C and forms a stable glass. Beginning with the work of Thomalia [17] in 1986, starburst molecules (dendrimers) have achieved enormous interest within the last years. Dendrimers are highly branched regular molecules, which are usually prepared by stepwise reactions. In many cases the behaviour of dendritic macromolecules are different from that of linear polymers, e. g. the former 23
2
Novel Photoconductive Polymers
usually show enhanced solubility. The reasons for these differences are the unique three-dimensional structure and the large number of chain ends in dendrimers. Two different methods have been developed for the stepwise synthesis of starburst dendrimers: a) the divergent approach, where the synthesis starts from a core molecule with two or more reactive groups; b) the convergent approach, in which the synthesis starts at the outer sphere of the dendrimer. In the divergent approach, the reaction of the core molecule with two or more reagents containing at least two protected branching sites is followed by removal of the protecting groups and subsequent reaction of the liberated reactive groups which leads to the starburst molecule of the 1st generation. The process is repeated until the desired size is reached. In the convergent approach the synthesis starts at what will become the outer surface of the dendrimer. Step by step large dendrimer arms are prepared and finally the completed arms are coupled to the core. Both methods produce well-defined large dendritic molecules whose structures are manifolds of the building blocks. They allow structural as well as functional group variation. On the other hand, hyperbranched polymers can be synthesized in a one-step reaction using highly functionalized monomers of the type AxB, where x is 2 or larger. This method does not yield polymers of such a well-defined structure, but has the advantage to provide rapidly large quantities of material. The control of the degree of branching is difficult and mainly depends on statistics, steric effects, and the reactivity of the functional groups. The aim of our work is the synthesis of starburst compounds with oxadiazole moieties. In contrast to the triphenylamine and carbazole derivatives oxadiazoles are strong electron acceptors. Therefore their transport characteristics can be switched from hole transport materials like 2,5-(4-diethylaminophenyl)-oxadiazole 1, in which the electron withdrawing effect of the oxadiazole ring is overcompensated by the two electron donating amino groups, to electron transport materials like 2-(biphenyl)-5-(4-tert.butylphenyl)-oxadiazole (PBD) 2. Recently, Saito demonstrated that oxadiazoles in a polycarbonate matrix show electron transport with mobilities up to 10 –5 cm2/Vs [18]. Such electron transport materials are attractive for the use in copiers and in organic light-emitting diodes.
2.3.2 Synthesis of starburst oxadiazole compounds Starburst oxadiazole compounds have been mentioned for the first time in a thermodynamic study of the structure-property-relationship in low molecular weight organic glasses [19, 20]. Upon rapid cooling these compounds form glasses with Tgs between 77 and 169 8C. We have used three different approaches for the preparation of starburst oxadiazole compounds, which are schematically shown in Fig. 2.2. The methods A and B can be compared to the divergent synthesis of dendrimers. Method A starts from a central core and involves the reaction of the acid chloride groups and a subsequent cyclisation with phosphorous oxychloride to the oxadiazole ring (Chap24
Cl
O
O
C
C
Cl
C O
Cl
Method B
Method A O H 2N
O C
NH
NH
O
O
C
C
O
NH
C
O NH
NH
C
C C
NH
N
NH O
N N
NH
C
N
N
N
O
N O
O
N N
= core
= shell
Method C
X
Z
+ X
X =
Y
X
OH ,
C
Z
CH
= core
Y =
Br ,
F
Z =
O
, C
Z
C
= shell
Figure 2.2: The different approaches to starburst oxadiazoles.
25
2
Novel Photoconductive Polymers
ter 1). The main difficulty in this case is that three functional groups must react in one step. Partially incomplete cyclisation causes problems, because the products contain one or two bishydrazides and are difficult to separate from the target compounds, which have three oxadiazole groups. Therefore we recently developed a totally different route (method B). The compounds 31 a–f were prepared by the reaction of benzene tricarbonyl chloride 30 with the tetrazoles 29. The latter were synthesized from benzonitriles 28 with potassium azide (Scheme 2.5). With the loss of nitrogen the tetrazole ring is transferred to the oxadiazoles [21]. This gives an easy access to unsymmetrically substituted oxadiazoles which we used for the first time in the synthesis of starburst oxadiazole compounds. In the third approach (method C) which is similar to the convergent synthesis a preformed oxadiazole precursor is prepared by stepwise synthesis and finally coupled to the core molecule. R1
R1
R2
CN
+
NH4Cl
NaN3
R3
N
R2
C N
R3
28
Cl
N
29
O
O
C
C
R1
Cl +
C O
NH
3
R2
N C N
R3
NH N
31a-f
pyridine
31a-f 2h, reflux
Cl
30
29
Scheme 2.5: Synthesis of starburst oxadiazoles via tetrazole intermediates.
For the preparation of the novel starburst molecules, different core molecules have been used: 1,3,5-benzene tricarboxylic acid chloride, 1,3,5-tris(4-benzoyl)benzene, 1,3,5triethynylbenzene, and 4,4',4@trihydroxytriphenylamine. Except benzenetricarboxylic acid which is commercially available, all core molecules were synthesized following well-known literature procedures [22, 23]. The structures of the starburst oxadiazole compounds are summarized in Tab. 2.3. 31 c and 31 g have been described before [19, 20], but no synthetisis procedure was given. The oxadiazoles 31 a–h have been prepared according to method B (Fig. 2.3), starting from benzene tricarboxylic acid chloride. Compound 31 g with tert.-butyl substituents was synthesized by method A, too. So a comparison of methods A and B is possible. The tetrazole route (method B) exhibits several advantages compared to the ring closure with dehydrating agents (method A). One advantage is the short reaction time. The reaction is finished within 2 hours whereas heating for 1–3 days is necessary if the ring closure is carried out with phosphorous oxychloride. Even more important is the facile work up procedure. In the case of the dehydration with POCl3 column chromatography and subsequent recrystallization is necessary to purify the product which is finally obtained in 33 % yield. In contrast only one filtration on a short silica gel 26
2.3
Starburst oxadiazole compounds
Table 2.3: Structures of the starburst oxadiazole compounds 31–34. Core a)
Comp.
Shell a)
N
31 a 31 b 31 c 31 d 31 e 31 f 31 g 31 h
R1
N
31
R2
O
R3
N
32
N
C
C
R = C(CH3)3
R
O
C
R1 = R3 = H, R2 = CH3 R2 = R3 = CH3, R1 = H R1 = R3 = CF3, R2 = H R1 = R3 = H, R2 = C2H5 R1 = R3 = H, R2 = OC2H5 R1 = R3 = H, R2 = CH(CH3)2 R1 = R3 = H, R2 = C(CH3)3 R1 = R3 = H, R2 = N(C2H5)2
C N
33
N R
O
R = C(CH3)3
C C
N
34
N
O
N O
R
R = C(CH3)3
a) cf. Figure 2.2.
column is sufficient for the purification of 31 g, prepared by the tetrazole route. In this case the yield of the pure product is 69 %. The starburst oxadiazole 32 has been prepared by method B too, whereas for 33 and 34 method C (Fig. 2.2) was used. The identity of all compounds was confirmed by NMR and FTIR spectroscopy.
2.3.3 Thermal properties The thermal behaviour of the starburst molecules has been investigated by differential scanning calorimetry and thermogravimetric measurements. 27
2
Novel Photoconductive Polymers
Table 2.4: Thermal properties of the starburst compounds 31–34. Compound
Molecular mass [g/mol]
Tg a) [8C]
Tm a) [8C]
Tdec b) [8C]
31 a 31 b 31 c 31 d 31 e 31 f 31 g 31 h 32 33 34
553 595 919 595 643 637 679 724 907 979 1122
– – – – 108 97 142 128 165 – 137
334 333 250 276 259 225 257 299 297 320 –
348 358 336 360 337 349 366 329 409 356 391
a) 3rd heating, determined by DSC with 20 K/min b) onset of decomposition in nitrogen, thermogravimetric measurement with 10 K/min
Among the compounds 31 a–h with a small benzene core both crystalline and glass forming materials exist. So 31 a–d with small methyl, ethyl, or trifluoromethyl substituents show only melting points in the DSC experiment with cooling rates of 20 K/min. Naito and Miura reported that it is possible to obtain glasses even with small methyl or trifluoromethyl substituents if the compounds are rapidly cooled with liquid nitrogen [19]. In contrast, the compounds 31 e with ethoxy, 31 f with iso-propyl, 31 g with tert-butyl substituents, and 31 h with diethylamino groups form glasses upon cooling with 20 K/min in the DSC equipment. When the amorphous samples are heated again the glass transition appears first but on further heating the samples start to recrystallize and consequently show a melting point at higher temperatures. Compound 32 with the triphenylbenzene core behaves similar like 31 e–h. The most stable glasses are formed by 34 with the triphenylamine core. The DSC diagram of the novel glass forming oxadiazole compound is shown below. Upon both, heating and cooling, only a glass transition is observed at 137 8C (Fig. 2.3). In our DSC experi-
Figure 2.3: DSC scan of the starburst oxadiazole compound 34, 3rd heating and cooling, with 20 K/min.
28
2.3
Starburst oxadiazole compounds
ments we never found any evidence for crystallization of 34. Even in the first heating no melting point is observed up to 350 8C. Consequently, transparent amorphous films are obtained from the starburst oxadiazole compound 34 by solvent casting. The thermal behavior of compound 33 is somewhat different. No reproducible DSC scans are obtained in subsequent heating-cooling cycles. We attribute this to thermal crosslinking of the triple bonds [24]. The thermal stability has been monitored by thermogravimetric measurements. In most cases the onset of decomposition is in the range from 330–370 8C. The oxadiazole compound 32 with a triphenyl benzene core shows a somewhat higher thermal stability up to 410 8C. (CH3)3C
N
N
N
N
C(CH3)3
O
O O
O N
O
N
O
N
C(CH3)3
34
The starburst oxadiazole compounds are now being tested as electron injection and transport layer in organic LEDs and as photoconductors. First tests of two layer LEDs with PPV show that the novel materials possess properties comparable to 2 but have the great advantage to show no recrystallization if thin films were made by spin-coating. We will report on these measurements in the near future.
29
2
Novel Photoconductive Polymers
References
1. H. Hoegl, O. Süs, W. Neugebauer, Kalle AG: DBP 1 068 115, Chem. Abstr., 55, 20742 a (1961), H. Hoegl: J. Phys. Chem., 69, 755 (1965) 2. W. Wiedemann: Chem.-Ztg., 106, 275 (1982) and references therein 3. A.R. Brown, D.D.C. Bradley, J.H. Burroughes, R.H. Friend, N.C. Green-ham, P.L. Burn, A.B. Holmes, A. Kraft: Appl. Phys. Lett., 61, 2793 (1992) 4. E. Buchwald, M. Meier, S. Karg, W. Rieß, M. Schwoerer, P. Pösch, H.-W. Schmidt, P. Strohriegl: Adv. Mater., 7, 839 (1995), M. Greczmiel, P. Pösch, H.-W. Schmidt, P. Strohriegl, E. Buchwald, M. Meier, W. Rieß, M. Schwoerer: Makromol. Symposia, 102, 371 (1996) 5. W. Warta, R. Stehle, N. Karl: Appl. Phys., A 36, 163 (1985) 6. P.M. Borsenberger, D.S. Weiss: in: Organic Photoreceptors For Imaging Systems, M. Dekker, New York, (1993) 7. R.G. Müller: PhD thesis, Bayreuth, (1992) 8. D. Girdziunaite, C. Tschierske, E. Novotna, H. Kresse, A. Hetzheim: Liq. Cryst., 10, 397 (1991) 9. F.H. Kreuzer, D. Andrejewski, W. Haas, N. Häberle, G. Riepl, P. Spes: Mol. Cryst. Liq. Cryst., 199, 345 (1991) 10. D. Adam, F. Closs, T. Frey, D. Funhoff, D. Haarer, H. Ringsdorf, P. Schuhmacher, K. Siemensmeyer: Phys. Rev. Lett., 70, 457 (1993) 11. D. Adam, P. Schuhmacher, J. Simmerer, L. Häussling, K. Siemensmeyer, K.H. Etzbach, H. Ringsdorf, D. Haarer: Nature, 371, 141 (1994) 12. M. Gailberger, H. Bässler: Phys. Rev. B, 44, 8643 (1991), M.A. Abkowitz, M.J. Rice, M. Stolka: Phil. Mag. B, 61, 25 (1990) 13. M. Stolka, J.F. Yanus, D.M. Pai: J. Phys. Chem., 88, 4707 (1984) 14. P.M. Borsenberger, L. Pautmeier, R. Richert, H. Bässler: J. Phys. Chem., 94, 8276 (1991) 15. C. Beginn, J.V. Grazulevicius, P. Strohriegl, J. Simmerer, D. Haarer: Macromol. Chem. Phys., 195, 2353 (1994) 16. Y. Kuwabara, H. Ogawa, H. Inoda, N. Noma, Y. Shirota: Adv. Mater., 6, 677 (1994) 17. D.A. Tomalia, H. Baker, J. Dewald, M. Hall, G. Kallos, S. Martin, J. Roeck, J. Ryder, P. Smith: Macromolecules, 19, 2466 (1986) 18. H. Tokuhisa, M. Era, T. Tsutsui, S. Saito: Appl. Phys. Lett., 66, 3433 (1995) 19. K. Naito, A. Miura: J. Phys. Chem., 97, 6240,(1993) 20. S. Egusa, Y. Watanabe: EP 553 950 A2 to Toshiba Corp. 21. R. Huisgen, J. Sauer, H.J. Sturm, J.H. Markgraf: Chem. Ber., 93, 2106 (1960) 22. E. Weber, M. Hecker, E. Koepp, W. Orlia, M. Czugler, I. Csöregh: J. Chem. Soc., Perkin Trans. II, 1251 (1988) 23. S.J.G. Linkletter, G.A. Pearson, R.I. Walter: J. Am. Chem. Soc., 99, 5269 (1977) 24. S.-C. Lin, E.M. Pearce: in: High-Performance Thermosets – Chemistry, Properties, Applications, Carl Hanser Verlag, Munich, 137 (1994)
30
3
Theoretical Aspects of Anomalous Diffusion in Complex Systems Alexander Blumen
3.1
General aspects
Many relaxation phenomena in the solid phase depend on diffusion, which is usually treated in the framework of statistical methods. Regular diffusion, known as Brownian motion, is characterized by a linear increase of the mean-squared displacement with time. On the other hand, for a whole series of phenomena this simple relation does not hold; their temporal evolution of the mean-squared displacement is non-linear and thus obeys at long times:
2 r
t t
1
with g 0 1. Relation 1 is referred to as anomalous diffusion. In the case that g < 1 one denotes the behaviour as subdiffusive. A subdiffusive pattern of motion often results from disorder [1–4]. One has to note, however, that the asymptotic law, Eq. 1, emerges only when the disorder influences the motion on all scales. In the case that g > 1 the motion is termed superdiffusive. A classical example for superdiffusive behaviour is furnished by the motion of particles in a turbulent flow. In this paper we focus on several models for anomalous diffusion which involve polymeric systems. Now, the mean-squared displacement is a basic characteristic feature for the motion but, as an averaged quantity, it can provide only restricted information about the basic microscopic mechanisms involved. In several works we have also studied the propagator P(r,t), the probability to be at r at time t having started at the origin at t = 0. Space limitations prevent us from going into details. Here we focus on Ar2 (t)S and refer to Klafter et al. and Zumofen et al. [4, 5] for in-depth analyses of the propagator. From the beginning, the role of time-dependent aspects in disordered media has to be emphasized. In usual random walk problems it is often assumed that the disorder is quenched, so that the dynamics evolves over a static substrate, i. e. the geometrical or the energetical disorder is frozen in. However, it is also possible that the dynamical processes are directly under the influence of temporal (possibly medium induced) fluctuations. First, in Section 3.2 we concentrate on photoconductivity, whose canonical description involves the continuous time random walk (CTRW) approach [1, 4, 6–8]. Basic ingredients Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
31
3
Theoretical Aspects of Anomalous Diffusion in Complex Systems
in CTRWs are waiting time distributions with long time-tails. For photoconductivity one usually has g < 1. Second, in Section 3.3 we display the Matheron-de-Marsily (MdM) model, in which particles move under the influence of external, randomly quenched flow fields [9–11]. Here, depending on the correlations between distinct field lines, superdiffusive behaviour with g > 1 shows up. An interesting dynamical feature is observed when the object to move has itself an internal structure; that is the case, for instance, for a polymer. In this case, because of the connections which exist between different segments of the polymer, the motion gets a very rich structure. The details of this situation will be discussed in Section 3.4. Finally, we close in Section 3.5 with some conclusions.
3.2
Photoconductivity
A major field of application of scaling ideas in the time domain is photoconductivity [1–3, 7, 12]; here the use of polymeric photoconductors in printing and copying represents one of the most sophisticated applications for organic materials. Such materials are nowadays superior to their inorganic counterparts. Now, the issue at stake in amorphous photoconductors is the appearance of dispersive transport, as contrasted to the familiar diffusive Gaussian behaviour. One observes experimentally that the motion of the charge carriers becomes slower and slower with the passage of time, a situation mirrored by Eq. 1 with g < 1. Introducing the diffusion coefficient D as the first derivative of Ar2 (t)S with respect to time one has from Eq. 1 an algebraic decay (since g < 1) of the form D
t t 1 :
2
Also the current I (t) which flows under the influence of an external field often depends algebraically on time. Here charge carriers, generated by a short light pulse, move through the sample and give rise to a transient photocurrent in the external circuit. Under this time-of-flight technique two regimes can be distinguished. For times shorter than the transit time tT (the time needed by the fastest carriers to cross the sample) the current obeys I t
1
;
3
whereas for t > tT one finds I t
1
:
4
For instance measurements on polysiloxanes with pendant carbazole groups [13] follow Eqs. 3 and 4 with g = 0.58 very well over four decades in time, see below. In fact this is 32
3.2
Photoconductivity
typical for g significantly lower than one. However, one should note that the behaviour of I (t) is complex, since for g > 1 in the long-time limit the transport behaviour is non-dispersive. This is related to the existence of a finite mean waiting-time t = g/(g – 1). It follows that around g = 1 there is a crossover from dispersive to non-dispersive behaviour [13], as is also confirmed experimentally. From the preceding discussion it is obvious that the transport of charge carriers is much influenced by the waiting-time distributions (WTD) between hops. Physically the WTD arise from the local disorder in the sample. For large disorder the WTD are not exponential but decay much more slowly. In line with the preceding arguments one takes for the WTD expressions c (t) which behave at long times algebraically [7, 12] 1
t t
;
5
where 0 < g < 1. This choice for c (t) reproduces Eqs. 2–4, see below. Equation 5 is not valid near the time-origin. Therefore in calculations one prefers to work with functions welldefined for t 6 0. A suitable choice is for instance the series
t
1 aX
1 a
an bn exp
bn t
6
n1
with a < 1 and b < a –1 [8]. This function is everywhere continuous and finite, and for purely imaginary t it turns into the Weierstrass function. One verifies readily that for large t Eq. 6 obeys Eq. 5 and that the corresponding g in Eq. 5 is g = ln a/ln b. Equation 6 is very useful, since it allows to vary g freely by a judicious choice of a and b. Another choice for c (t) which is continuous for t 6 0 is
t
1 t :
7
Here again the long-time behaviour follows Eq. 5. We now recall the basic ingredients of random walks in continuous time, the so-called CTRW [6–8]. Let c (r, t) be the probability distribution of making a step of length r in the time interval t to t + dt. The total transition probability in this time interval is
t
X
r; t:
8
r
Furthermore the survival probability at the initial site is
t 1
Rt 0
d;
9
so that, switching to the Laplace space (t ? u), one has
u 1
u=u:
10 33
3
Theoretical Aspects of Anomalous Diffusion in Complex Systems
The probability density Z (r, t) of just arriving at r in the time interval t to t + dt obeys the iterative relation
r; t
P Rt r0 0
r0 ;
r
r0 ; t
d
t r;0 ;
11
in which the initial condition of starting at t = 0 from r = 0 is incorporated. One then has for the probability P (r,t), that the particle is at r at time t, P
r; t
Rt 0
r; t
d:
12
Now P (r, t) also obeys an iterative relation: P
r; t
X Rt r0
0
P
r0 ;
r
r0 ; t
d
t r;0
13
as may be seen either by inspection or, more formally, by using Eqs. 11 and 12. Clearly, a description of such convolutions, Eqs. 11–13, is more compact in Fourier-Laplace space. For P (k, u) one has from Eq. 13: P
k; u P
k; u
k; u
u
14
with the immediate solution P
k; u
u=1
k; u
1
u u
1
1 :
k; u
15
The last expression generalizes the usual diffusion relation to random media, in which spatial and temporal aspects are coupled through c (k, u). The analysis is much simplified if such aspects decouple, which is the case for instance when the disorder is mainly energetic and the random walker moves over a rather regular lattice. In the decoupled case:
r; t
r
t :
16
From this it follows immediately that also c (k, u) = l (k) c (u) is decoupled. In the decoupled scheme P (k, u) takes the form P
k; u
1
u u
1
1
k
u
;
17
P where l (k) = q p (q)e–ik7q is the structure function of the infinite lattice and p (q) denotes the probability that a step extends over the distance q. 34
3.2
Photoconductivity
Coupling is very important for superlinear behaviour. Thus for the c (r, t) given by Eq. 16 the mean-squared displacement is either divergent or increases sublinearly or at most linearly in time. In order to obtain finite Ar2 (t)S with a superlinear temporal behaviour, coupled c (r, t) forms have to be used [4]. An example is the WTD
r; t Ar
r
t ;
18
in which the d-function couples r and t. This WTD leads to Lévy walks. Let us now focus on the mean-squared displacement. Evidently, one has
R r2
t r2 P
r; t dr
rk2 P
k; t jk0
19
from which, in the decoupled scheme, using Eqs. 5 and 17 it follows that in the absence of any bias Eq. 2 is fulfilled. The procedure is more readily examplified by calculating the current from the mean displacement of the carrier Ar(t)S in a biasing field [8]. Setting L –1 for the inverse Laplace transform it follows:
P r
t rP
r; t irk P
k; t k0 L 1
irk P
k; ujk0 r
@ P
k; u
u 1 j q ; L 1 L ir
k k k0 @ u 1
u 1
20
P where in the last line we work in the decoupled scheme and AqS = q qp (q) is the mean displacement per hop. In the presence of a bias AqS 0 0. Thus, setting |AqS| = 1, we have for the current I (t) in an infinite lattice of any dimension, d r
t 1 L I
t 1 dt
u :
u
21
For a finite chain of N sites Eq. 21 takes in the Laplace space the form [3, 13]: I
u
N X n1
un
1
u 1
u
uN :
22
It is precisely this function which was used in Refs. [13, 14] to analyse, together with the WTD Eq. 6, the time-of-flight currents of photoconductive carriers in polysiloxanes with pendant carbazole groups. In this work one achieved with g = 0.58 a good agreement with the experimental findings. The short time behaviour indeed obeys Eq. 3, whereas at long times the form of Eq. 4 is reproduced fairly well.
35
3
3.3
Theoretical Aspects of Anomalous Diffusion in Complex Systems
The Matheron-de-Marsily model
As mentioned in the introduction, superdiffusive (enhanced) behaviour is often found in turbulent flows. In this Section we adopt a picture different from CTRW. We focus on the influence of randomly distributed biasing external fields and follow the description of Oshanin and Blumen [11]. We take a three-dimensional (3D) solvent for which the flow is parallel to the Y-axis. The direction and magnitude of the flow depend only on the X coordinate of the position vector [9] so that VY, the non-vanishing component of the flow field, obeys: VY
X; Y; Z V X :
23
Here furthermore V[X] is a random function of X. Geometrically the system consists of parallel layers perpendicular to the X-axis. In each layer the value of VY is constant but varies from layer to layer [9]. We assume the random function V[X] of Eq. 23 to be Gaussian with zero mean, AV[X]S = 0, and with the covariance
V X1 V X2
jX1
X2 j:
24
Here the brackets denote configurational averages, which are conveniently expressed through Fourier integrals,
j X1
X2 j
R1 1
dwQ
w exp iw
X1
X2 :
25
Now many possibilities for Q (w) can be envisaged. For simplicity we take here only a flat spectrum, Q (w) = W/2p, as in the original Matheron-de-Marsily (MdM) model [9] in which the flows are delta-correlated,
jX1
X2 j W
X1
X2 :
26
We start from the Langevin dynamics of a single spherical bead subject to the MdM flow. This allows us to display enhanced (superlinear) diffusion in a simple situation [9, 10, 22]. The study of the dynamics of Rouse polymers in such flows is deferred to the next Section. Let R (t) be the position of the center of mass of the bead at time t, and we assume that R (0) = 0. The components X(t), Y(t) and Z(t) of R(t) obey the following Langevin equations
36
m
d2 X dt2
dX fX
t ; dt
27
m
d2 Z dt2
dZ fZ
t ; dt
28
3.3
d2 Y m 2 dt
dY dt
The Matheron-de-Marsily model
V X fY
t :
29
Here m denotes the mass of the bead and z the friction constant. The terms fX (t), fY (t), and fZ (t) give the random (thermal-noise) forces exerted on the bead by the solvent molecules. These forces are Gaussian, with the moments f i
t 0
30
and fi
t fj
t0 2 T i;j
t
t0 ;
31
where i,j B {X,Y,Z}. The dash stands for thermal averaging, di,j is the Kronecker-delta and the temperature T is measured in units of the Boltzmann constant kB . Conventionally the acceleration terms in Eqs. 27–29 are neglected, since they are small relative to the other terms [15]. This leads to
dX fX
t ; dt
32
dZ fZ
t ; dt
33
dY VX
t fY
t : dt
34
Note that in Eq. 34 the X and Y coordinates are coupled. Equations 32 and 33 are readily solved, X
t
1
Z
t
1
Rt
d fX
;
35
d fZ
:
36
0
Rt 0
Thus the bead undergoes a conventional diffusive motion between the layers (along the X-axis) and in the Z direction. One sees it readily by evaluating, say:
X 2
t
2
Rt 0
Rt Rt Rt d1 d2 fX
1 fX
2 2 1 T d1 d2
1 0
0
0
2 2
T= t ;
37
so that X 2
t 2D1 t, where D1 = T/z is the diffusion coefficient of a single bead. 37
3
Theoretical Aspects of Anomalous Diffusion in Complex Systems
A similar procedure can be performed with respect to the solution of Eq. 34, Y
t
Rt 0
d V X
1
Rt 0
d fY
:
38
The averaging involves now both, the thermal noise and the configurational disorder: Y 2
t
2
Rt 0
Rt Rt Rt
d1 d2 fY
1 fY
2 d1 d2 VX
1 VX
2 0
0
2D1 t
W=2
Rt 0
0
Rt R1 d1 d2 dw exp iw
X
1 1
0
X
2 ;
39
where in the last line use was made of the representation Eqs. 25 and 26 with the flat spectrum of the delta-function. The remaining average on the rhs. of Eq. 39 is readily evaluated by remembering that it is the characteristic functional of the Brownian trajectory
1 ; 2 ; w exp iw
X
1
X
2 exp
w2 D1 j1
2 j :
40
Inserting Eq. 40 into Eq. 39 one recovers the following result for the average squared displacement (ASD) in the direction of the flow field,
4W Y 2
t 2 D1 t 3
t3 p D1
1=2 :
41
One should remark that at times greater than tc = 9 pD31/(4W2) the superlinear growth t3=2 in Eq. 41 dominates and the first, diffusive term can be neglected. One has then a superdiffusive behaviour with an exponent of g = 3/2 in Eq. 1 [9]. We now turn to the analysis of the behaviour of polymers in MdM flow fields. hY 2
ti
3.4
Polymer chains in MdM flow fields
The conformational properties and the dynamics of polymers in solutions under various types of flows have been a subject of considerable interest within the last decades. Much progress has been gained in the explanation of experimental data for systems in which the flow velocities are given functions in space and time, see Refs. [16–19]. On the other hand, the behaviour of polymers in random flows is less understood. In recent works [11] we (Oshanin and Blumen) succeeded in establishing analytically the behaviour of Rouse polymers [20] in MdM flow fields. The presentation here follows closely Ref. [11]. 38
3.4
Polymer chains in MdM flow fields
In the Rouse model N monomers (beads) are coupled to each other via harmonic springs [16, 17, 20]. As is well-known, the forces are of entropic origin. It is customary to revert to a continuous picture in which n, the bead’s running number, takes real values. For a detailed discussion see Doi and Edwards [17]. The Langevin equations of motion for such a polymer in the MdM flow field are
@ Xn
t @2 Xn
t K fx
n; t ; @t @ n2
42
@ Zn
t @2 Zn
t fZ
n; t ; K @t @ n2
43
@ Yn
t @2 Yn
t K VXN
t fY
n; t ; @t @ n2
44
see Ref. [11]. Equations 42–44 are the generalization of Eqs. 27–29 to polymers. They are to be solved subject to the Rouse boundary conditions at the chain’s ends, n = 0 and n = N [17]: @ Xn
t @ Yn
t @ Zn
t 0: @n @n @n
45
As before, the fluctuating forces on the rhs. of Eqs. 42–44 are Gaussian and also delta-correlated with respect to the running index [11, 17]. For the X and Z components, which are not subject to the flow, the procedure is standard [17]. Say, for the averaged X component of the end-to-end vector one has P2X
t
X0
t
XN
t2
b2 N ; 3
46
where b is the so-called persistence length. Furthermore, the X component of the radius of gyration is Xg2
1 2N 2
ZN ZN dn dm
Xn
t 0
0
Xm
t2
b2 N : 18
47
For isotropic situations (in the absence of flow fields) the end-to-end vector PR and the radius of gyration Rg of the polymer are related to PX and Xg through P2R = 3P2X and R2g = 3X 2g . Because of the anisotropy one has to consider in the MdM model the different components separately. The dynamics of a flexible polymer chain is richer than that of a single bead. In the Rouse model the dynamics of Xn (t) depends essentially on the time of observation t and on the Rouse time tR, R
b2 N 2 : 3p2 T
48 39
3
Theoretical Aspects of Anomalous Diffusion in Complex Systems
Now tR is the largest internal relaxation time of the chain [17, 20]. Exemplarily for t P tR one finds for the mean-squared displacement of a bead of the chain, say the zeroth one,
X0
t
X0
02 2b
D1 t 3p
1=2
:
49
Equation 49 is subdiffusive with g = 1/2 in Eq. 1. This is due to the fact that the trajectory of a bead in a chain is spatially confined by its neighbours. In the limit t p tR the chain diffuses as one entity and the bead’s trajectory follows mainly the motion of the chain’s center of mass. The chain’s center of mass obeys X 2
t 2DR
N t
50
with DR (N) = D1/N { T/(zN). Let us now turn to the Y component of the center of mass for which Eq. 44 leads readily to 1 Y
t N
ZN 0
ZN
Zt
1 dnYn
t N
d 0
dn V Xn
1 fY
n; ;
51
0
so that we obtain
W Y 2
t 2DR
N t 2N
Zt
Zt d1
0
Z1 dw g
w; 1 ; 2 ;
d2
52
1
0
where g(w; t1, t2) denotes the dynamic structure factor of the chain, 1 g
w; 1 ; 2 N
ZN ZN dn dm exp iw
Xn
1 0
Xm
2 :
53
0
It turns out [11], that all these integrations can be performed analytically. In the longtime limit t p tR one finds
4W Y 2
t 2DR
N t 3
N pT
1=2
t3=2 1
O
t
1=2
;
54
whereas for t P tR the short-time behaviour is given by
Y 2
t 2DR
N t 40
p 3 W 2 t 1 bN 1=2
O
t
1=4
:
55
3.4
Polymer chains in MdM flow fields
The interpretation of Eq. 54 is that at long times the t3/2 dynamics dominates the picture; the Rouse chain behaves like a compact bead. At short times the term t2 may become important. This g = 2 case in Eq. 1 is called ballistic; at very short times the center of mass of the chain hardly moves and it practically does not change the flow pattern to which it is subjected. We remark that at short times the motion of the center of mass of the chain and the motion of a tagged bead are characterized by different dependences on time. The mean-squared displacement along the Y-axis of a tagged bead, say the zeroth one, grows in time as
2 W Y0
t e2DR
N t 1=2 D1 1=4 t7=4 ; b
56
see Ref. [11]. This g = 7/4 dependence is, of course, related to the fact that the segmental motion at short times is confined, the number of distinct flow layers visited by the bead growing as t1/4. Results of such fractal-type behaviour may be formulated exactly [21, 22]. We now turn to the question of the elongation of the Rouse chain in the MdM flow and sketch the evaluation of the end-to-end distance along the Y-axis [11]. The solution of Eq. 44 under the boundary conditions Eq. 45 has the form of a Fourier series, Yn
t Y
0; t 2
1 X
cos
ppn
p1
N
Y
p; t ;
57
where the Y (p,t), p = 0, 1, …, denote the normal coordinates [17]. At t = 0 the chain is assumed to be in thermal equilibrium, i. e. to have a Gaussian conformation. This can be accounted for automatically by stipulating it to be subject to the thermal fluctuations since t = –?. Furthermore, the MdM flow fields are switched on at t = 0. This leads to Y
p; t 1 N
Zt
Rt 1
dn cos 0
=R f~Y
p;
d exp
p2
t
ZN d
0
1
ppn N
VXn
t
exp
p2 =R ;
58
where the functions f~Y denote the Fourier components of the thermal fluctuations [17]. The Y component of the end-to-end vector follows now from: PY
t Y0
t
YN
t 2
1 P p1
1
1p Y
p; t :
59
After performing the averaging over both, the thermal fluctuations and the realizations of the flow fields, one obtains from Eqs. 58 and 59 in the long-time limit the equilibrium value of the end-to-end vector for delta-correlated flows [11], 41
3
Theoretical Aspects of Anomalous Diffusion in Complex Systems
2 b2 N CW2 bN 5=2 1 PY
1 ; 3 T2
60
where C is a constant. Therefore, a Rouse polymer stretches along the Y-axis under MdM flows, taking the form of a prolate ellipsoid. The correction term to the Gaussian behaviour grows as N7/2. It is now interesting to confront this finding with the situation in simple shear flows, for which the result is [18, 19]: P2Y
t
b2 N 3 _ 2 2 b4 N 4 1 : 3 6480 T2
61
In Eq. 61 _ stands for the (constant) shear rate. Because all flow lines point now in the same direction, the correction term shows a stronger N-dependence and obeys a N5 law.
3.5
Conclusions
In this review several situations were presented, which lead naturally to the appearance of anomalous diffusion. Besides the already well-discussed subdiffusive behaviour, which is often seen in disordered media, we also considered superdiffusive dynamics, such as encountered in layered random flows. Anomalous diffusion was analysed through several models and we focussed on the behaviour of polymeric materials under such conditions. The basic aspect underlying these phenomena is dynamical scaling, which is often encountered experimentally and theoretically. On the other hand not all systems scale with time, and care is required in applying the models presented here; one has to be aware of intrinsic limitations of the scaling range (e. g. size limitations, other temporal scales involved). Because of this, close cooperations between experimentalists and theoreticians are much needed for the analysis of systems similar to the ones described here. Furthermore, despite the success of the now-closing Collaborative Research Center 213, much work still remains to be done.
Acknowledgements
The research collaboration with Prof. D. Haarer, Prof. J. Klafter, Dr. G. Oshanin, Dr. H. Schnörer, and Dr. G. Zumofen in our joint work reviewed here was always very helpful and pleasant. The support of the Deutsche Forschungsgemeinschaft through the Sonder42
References forschungsbereich 213 and Sonderforschungsbereich 60 was fundamental for the whole project. Additional help was provided by the Fonds der Chemischen Industrie and – in the later stages – by the PROCOPE-Program of the DAAD.
References
1. A. Blumen, J. Klafter, G. Zumofen: in: I. Zschokke (ed.): Optical Spectroscopy of Glasses, Reidel, Dordrecht, p. 199 (1986) 2. D. Haarer, A. Blumen: Angew. Chem. Int. Ed. Engl., 27, 1210 (1988) 3. A. Blumen, H. Schnörer: Angew. Chem. Int. Ed. Engl., 29, 113 (1990) 4. G. Zumofen, J. Klafter, A. Blumen: in: R. Richert, A. Blumen. (eds.): Disorder Effects on Relaxational Processes: Glasses, Polymers, Proteins, Springer, Berlin, p. 251 (1994) 5. J. Klafter, G. Zumofen, A. Blumen: J. Phys., A24, 4835 (1991) 6. E.W. Montroll, G.H. Weiss: J. Math. Phys., 6, 167 (1965) 7. H. Scher, M. Lax: Phys. Rev. B, 7, 4491; 4502 (1973) 8. M.F. Shlesinger: J.Stat. Phys., 36, 639 (1984) 9. G. Matheron, G. de Marsily: Water Resour. Res., 16, 901 (1980) 10. G. Zumofen, J. Klafter, A. Blumen: Phys. Rev. A, 42, 4601 (1990) 11. G. Oshanin, A. Blumen: Macromol. Theory Simul. 4, 87 (1995); G. Oshanin, A. Blumen: Phys. Rev. E, 49, 4185 (1994) 12. H. Scher, E.W. Montroll: Phys. Rev. B, 12, 2455 (1975) 13. H. Schnörer, H. Domes, A. Blumen, D. Haarer: Philos. Mag. Lett., 58, 101 (1988) 14. D. Haarer, H. Schnörer, A. Blumen: Dynamical Processes in Condensed Molecular Systems, in: J. Klafter, J. Jortner, A. Blumen (eds.): World Scientific, Singapore, p. 107 (1989) 15. M. Fixman: J. Chem. Phys., 42, 3831 (1965) 16. P.G. de Gennes: in: Scaling Concepts in Polymer Physics, Cornell Univ. Press, Ithaca, N.Y., (1979) 17. M. Doi, S.F. Edwards: in: The Theory of Polymer Dynamics, Oxford Univ. Press, Oxford, (1986) 18. R.B. Bird, C.F. Curtiss, R.C. Armstrong, O. Hassager: in: Dynamics of Polymeric Liquids, Vol.2, 2nd Ed. Wiley, New York, (1987) 19. W. Carl, W. Bruns: Macromol. Theory Simul., 3, 295 (1994) 20. P.E. Rouse: J. Chem. Phys., 21, 1273 (1953) 21. J.-U. Sommer, A. Blumen: Croat. Chem. Acta, 69, 793 (1996) 22. G. Zumofen, J. Klafter, A. Blumen: J.Stat. Phys., 65, 991 (1991)
43
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, Specific Heat and Thermal Conductivity in Polymers Andreas Nittke, Michael Scherl, Pablo Esquinazi, Wolfgang Lorenz, Junyun Li, and Frank Pobell
We have measured the long time (t = 5 h to 200 h) heat release of polymethylmethacrylate (PMMA) and polystyrene (PS) at 0.070 K ^ T ^ 0.300 K. After cooling from a temperature (the charging temperature) of 80 K the heat release in PMMA shows a t –1-dependence in the measured time and temperature ranges in agreement with the tunneling model. In contrast, for PS we observe strong deviations from a t –1-dependence and a heat release smaller than in PMMA in by a factor of ten, in apparent contradiction to specific heat and thermal conductivity data for PS. To compare the heat release with other low-temperature properties and to verify the consistency of the tunneling model we have measured also the acoustical properties (sound velocity and attenuation), the specific heat and the thermal conductivity of PMMA and PS in the temperature ranges 0.070 K ^ T ^ 100 K, 0.070 K ^ T ^ 0.200 K and 0.3 K ^ T ^ 4 K, respectively. We show that the anomalous time dependence of the heat release of PS is due to the thermally activated relaxation of energy states with excitation energies above 15 K.
4.1
Introduction
A disordered material releases heat after cooling it from an equilibrium or charging temperature T1 to a measuring temperature T0 [1]. This heat release Q_ (T1,T0, t) depends on the charging temperature T1 as well as on the temperature T0, at which the measurement is performed, and the elapsed time during and after cooling [2, 3]. The time-dependent heat release, observed in several disordered systems, is a consequence of the long-time relaxation of the low-energy excitations, identified as two-level tunneling systems (TS) [4–6]. As a consequence of the finite relaxation time of the TS through their interaction with thermal phonons [7] the specific heat depends also on the time scale of the experiment [5], as first measured by Zimmermann and Weber [1]. In recent publications [5, 6] it was shown that within the tunneling model we can quantitatively understand the observed temperature and time dependence of the specific heat 44
Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
4.1
Introduction
and heat release of vitreous silica (SiO2) over ten orders of magnitude in time. It has also been pointed out that the measurements of the heat release at workable long times is probably the only feasible method to obtain at least approximately the low-energy limit of the tunnel splitting D0 of the distribution function of TS. This low-energy limit is considered in the literature by the cut-off parameter umin = (D0 /E)min of the distribution function (E is the energy splitting of the TS) and is introduced to keep the number of TS finite, avoiding divergences in the calculated properties. The interpretation of the heat release data in terms of the tunneling model is a difficult task due to the not well-known: a) temperature and time dependence of the specific heat due to TS at T > 3 K; b) influence of relaxation processes of the TS at T > 3 K other than one-phonon tunneling relaxation, i. e. high-order phonon tunneling and thermally activated relaxation; c) influence of the cooling procedure. In a recently published paper Parshin and Sahling [8] showed the complexity of the interpretation of the heat release data when thermally activated relaxation is taken into account within the framework of the soft potential model. Further theoretical work on the residual properties of two-level systems and its dependence on the cooling procedure has been published by Brey and Prados [9]. In this paper we present a further example of the complexity in the interpretation of the heat release data and an experimental proof of the influence of the relaxation, probably by thermally activated processes, of excited states that contribute to the heat release of the TS at low temperatures. We have studied the long-time heat release of two amorphous polymers with similar low-temperature specific heats and thermal conductivities, cooled under similar conditions. In spite of those similarities we have found a large difference in the absolute value and in the time dependence of the heat release between the two polymers when cooled from temperatures above 15 K. The similarities and differences in the low-temperature properties, their interpretation within the tunneling model, and the influence of thermally activated relaxation are the main scope of this work. Preliminary results were published in Ref. [10]. The paper is organized in five sections. In Section 4.2 we describe the phenomenological theory for the heat release, based on the tunneling model and the influence of different relaxation rates, and the cooling process. In Section 4.3 we briefly describe the experimental procedures and samples. In Section 4.4 we show and discuss the experimental results. Conclusions are drawn in Section 4.5.
45
4
4.2
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
Phenomenological theory for the heat release
4.2.1 Generalities New theoretical work for the calculation of the heat release within the soft potential model has been published recently [8]. In order to simplify the calculations, to minimize the number of free parameters, and to assure a more transparent interpretation of the results we decided, however, to interpret our results in terms of the standard tunneling model. According to Ref. [8] and to our numerical calculations the differences between the soft potential and standard tunneling model are not significant at the low temperatures of our measurements. The standard tunneling model, including a thermally activated relaxation of the twolevel systems, was used successfully to interpret the acoustical properties of vitreous silica in eight orders of magnitude in phonon frequency from approximately 0.1 K up to room temperature [11]. For a system of N two-level systems with energy difference E, the difference in the population of the two levels at a given temperature T and at thermal equilibrium is given by n0 N tanh
E=2kB T :
1
If the thermodynamic equilibrium of the system is slightly perturbed, e. g. the system is rapidly cooled to a temperature T, the dynamical behaviour of the population difference can be calculated according to the relaxation time approximation formula: n0
T
d
n
t dt
n
t n0
T ;
E; T
2
where t (E,T) is the relaxation time of a tunneling system with energy E at a temperature T. The heat released by the N two-level systems after the temperature change is given by _ Q_ nE=2 :
3
The problem of calculating Q_ simplifies to calculating n from Eq. 2. However, the cooling process has to be taken into account. In this case Eq. 2 must be rewritten as n_
@n0 dT @T dt
n
n0
:
4
Equation 4 describes the response of two-level systems during a temperature change given by the function T (t). In the general case Eq. 4 has to be solved numerically since n0 and t are temperature-dependent variables.
46
4.2
Phenomenological theory for the heat release
4.2.2 The standard tunneling model with infinite cooling rate If N two-level systems are in thermal equilibrium at a temperature T1 and they are cooled to T0 with infinite cooling rate, i. e. the time to cool the sample from T1 to T0 is zero, from Eq. 2 we obtain n
t
n0
T1
n0
T0 exp
t=
E; T0 n0
T0 :
5
The standard tunneling model assumes that at low temperatures (T < 2 K) the one-phonon process is the dominating mechanism. The one-phonon relaxation rate is given by p 1 pm1 u2
6
pm1 AE 3 coth
E=2KB T ;
7
with
where A = (g 2l /n 5l + 2 g 2t n 5t )/2 pr–4. The indices l, t refer to the longitudinal and transversal phonon branches, r is the mass density, gl and gt are the coupling constants between phonons and TS, and u = D0 /E (D0 is the tunneling splitting). For symmetrical TS, i. e. D0 = E (u = 1), tp reaches its minimum value tpm . Furthermore, the standard tunneling model assumes that the distribution function of TS is constant in terms of two independent variables, namely the asymmetry D and the tunneling parameter l, i. e. P
; dd Pdd :
8
According Ref. [7] the distribution function can be written in terms of the variables E and u as
1 P
E; u P=u
u2 1=2 :
9
It is also convenient to have the distribution function in terms of the asymmetry and the barrier height V between the potential wells. Following the work of Tielbürger et al. [11] and assuming two well-defined harmonic potentials, it can be shown that in a first approximation l = V/E0 where E0 represents the zero-point energy. In this case the distribution function is P Pdd ddV : E0
10
Replacing the total number N of TS with the integrals in E and u, the heat release is given by 47
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
1 Z PV E Q_ dEE tanh E0 2kB T0 0
E tanh 2kB T1
Z1 umin
du p 1
T0 exp
t=
T0 ; u 1 u2 (11)
where V is the sample volume and umin is the cut-off in the distribution function at u ? 0. Figure 4.1 shows the heat release at T0 = 0.1 K as a function of time for different charging temperatures T1 following Eq. 11 and taking into account one-phonon relaxation rate, Eqs. 6 and 7. The calculation was performed with parameters appropriated for vitreous silica, Ak 3B = 46106 s–1 K–3, P = 1.661038 J–1 g–1 and umin = 5610–8 [5]. We observe that at short times and small T1 the heat release Q_ ! t–1 T 21. This dependence follows from the logarithmic time dependence of the specific heat and holds for t P tm/u2min . In this limit the heat release follows the often used approximation from Eq. 11 [1]: p2 2 Q_ k PV
T12 24 B
T02
1 ; t
12
where Q_ and P are measured in W and (Jg)–1. We recognize in Fig. 4.1, however, that at longer times the theory deviates from the t –1-dependence. This deviation comes from the exponential term in Eq. 11 that decreases strongly at long times and is determined by the product Au2min. The smaller this product the larger is the time-range where the approximation given by Eq. 12 holds. The influence of the cut-off umin can be recognized comparing the calculated heat release in Fig. 4.1 with that in Fig. 4.2 (dashed lines) calculated with a smaller umin. In Fig. 4.1 we note also that at large times the heat release becomes independent of T1. This feature was recognized experimentally in Refs. [2, 3] and was discussed in Ref. [6]. This T1-independence within the assumptions described above is a direct consequence of the finite number of TS given by the cut-off umin. We should note, however, that in SiO2 a saturation of the heat release for large charging temperatures (T1 > 20 K) is observed and still a t –1-dependence was measured [2]. This result cannot be explained within the standard tun-
Figure 4.1: Heat release as a function of time t (in s) according to the standard tunneling model and infinite cooling rate with Ak 3B = 46106 s–1 K–3, P = 1.661038 J–1 g–1 and umin = 5610–8 at a measuring temperature of 0.1 K and at different charging temperatures T1, bottom: 5 K, top: 80 K.
48
4.2
Phenomenological theory for the heat release
Figure 4.2: Heat release as a function of time t (in s) within the standard tunneling model and infinite cooling rate. The parameters are the same as in the previous figure but with umin = 5610–9 (dashed lines) and an additional constant (energy-independent) relaxation time tTA = 103 s (continuous lines).
neling model. The reason for this discrepancy is the relaxation rate, which is different from the one-phonon process at higher temperatures and the influence of a finite cooling rate (see below).
4.2.3 Influence of higher-order tunneling processes and a finite cooling rate At temperatures above 3 K tunneling processes of higher-order are, in principle, possible. One particular high-order process was studied theoretically in Ref. [12] and is similar to the optical Raman process; the relaxation time of the TS is given by an interaction that involves two phonons. Following Ref. [12] we added this Raman relaxation rate to the one-phonon relaxation rate (Eq. 6). Following Ref. [12] a new free parameter, i. e. the coupling constant R for the Raman process, is assumed. Due to its strong temperature dependence (T 7), the Raman process can influence the population difference of the energy states of the TS mainly at high temperatures (T > 5 K) during the cooling process. We should note that for infinite cooling rate and for the temperature range of our measurements (T0 ^ 1 K) the contribution of the Raman process to the time and temperature dependence of the heat release is negligible. This follows from Eq. 5 where only the relaxation of the TS at the measurement temperature T0 enters. In order to take into account the cooling process we used the algorithm explained below. The zero-time point is chosen as the time when the cooling process is started. The function n (E,u,t) represents the difference in population of the TS energy states at any time t and n0 (E,T) means this difference in equilibrium (t ? ?) at a temperature T. Analog to Eq. 11 the heat release can be written as: 1 Q_ PV 2
Z1 Z1 dEE 0
umin
du p 1
T0 e u 1 u2
1
T0 t
n0
E; T0
n
E; u; t 0
13
49
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
Note that the population difference n depends on E and u because the relaxation rates, that influence the relaxation of the TS, depend on these variables. As already described above, to obtain the function n we need to solve the differential equation given by Eq. 4. In general this is only possible by numerical methods. The time dependence of the temperature during the cooling process performed in this work can be well approximated by a linear function given by T
t T1
T0
T1 tA
:
14
We assume that the sample is at t = 0 (tA) at T1 (T0); tA is the time needed to cool the sample from T1 to T0. The calculations have been done splitting the function T (t) in N steps of time Dt (Fig. 4.3). During the time Dt the temperature remains constant and n (E,u,t) shows an exponential behaviour given by Eq. 5; this is qualitatively shown in Fig. 4.3. To obtain the population difference at the time Dt cooling from T1 at t = 0 for a given E and u we calculate iteratively the value n
t 0 t n0
0 t
n0
0 t
n
0 e
1
T
0tt
:
15
The calculations given in this work have been made taking into account 10 to 200 time-steps or iterations depending on the convergence of the numerical results. Figure 4.4 shows the heat release as a function of time taking into account one-phonon (dashed lines) and the Raman process (Rk7B = 100 s–1 K–7) with a cooling time tA = 3000 s from T1 to T0 = 0.1 K. Taking into account our experimental time scale the calculations were performed for the time interval 104 s ^ t ^ 106 s only. For one-phonon
Figure 4.3: Time dependence of the sample temperature during a cooling process and its splitting in N steps (dashed lines) assumed for numerical calculations. Bottom: qualitative behaviour of the population difference of the tunneling systems n0 (T) as a function of time.
50
4.2
Phenomenological theory for the heat release
Figure 4.4: Heat release as a function of time for a finite cooling time TA = 3000 s and with (continuous lines) or without (dashed lines) Raman processes.
process only, our calculations indicate that a finite cooling rate with tA = 3000 s to 5000 s has a negligible influence (< 3 %) on the heat release in our experimental time scale (compare the dashed lines in Fig. 4.4 with the dashed lines in Fig. 4.2 obtained with an infinite cooling rate). The influence of the Raman process at T0 = 0.1 K can be well observed if we take into account a finite cooling rate. In comparison with the results using the one-phonon process only and for T1 > 20 K, Q_ is smaller and shows a slightly different time dependence. Note that the results for T1 6 20 K resemble those obtained taking into account the one-phonon process only but with a smaller charging temperature T1. We note also that at T1 ^ 20 K the heat release still shows a T 21-dependence but reaches its saturation at a smaller T1 in comparison with the results with the one-phonon process only (Fig. 4.4). We conclude that taking into account Raman processes, that influence the relaxation rate of TS at temperatures larger than 2 K, it is possible to understand qualitatively the results of, for example, SiO2 where Q_ reached a saturation at T & 10 K but still shows a t –1dependence at t ^ 36105 s [2]. This result is only valid if the product Au2min in Eq. 7 remains small enough. Because of the uncertainty in the coupling constant R between TS and phonons a quantitative comparison, however, of the heat release results with the theory taking into account the contribution of higher-order processes is not useful. Phenomenologically and in order to simplify the calculations, one can take into account the influence of higher-order processes by choosing an appropriate smaller charging temperature than the real one. In that sense charging temperatures T1 6 10 K can be considered for comparison with theory as free parameters. From our calculation we learn that it is practically impossible to obtain reliable information on the density of states of TS from heat release experiments for charging _ temperatures in the region of the T1-saturation of Q.
51
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
4.2.4 The influence of a constant and thermally activated relaxation rate There are different attempts to link the high-temperature (T > 10 K) with the low-temperature properties of disordered solids [13, 14]. In particular, it has been proposed that the maximum in the attenuation of phonons observed in amorphous materials at T > 10 K can be interpreted assuming a thermally activated relaxation of the two-level systems. In this Section we discuss the influence of thermally activated relaxation rate on the heat release for a finite cooling rate. For a single activation barrier V0 between the two potential wells and at a measuring temperature T0 the thermally activated relaxation rate is given by TA1 0 1 e
V0 =kB T0
:
16
Taking into account this relaxation rate in addition to quantum tunneling (Eq. 6) and assuming that both processes are independent, the total relaxation rate can be written as
1
P 1 TA1 :
17
Obviously, at a given temperature T0 and for a single activation barrier we add a constant relaxation rate to the tunneling process. Figure 4.2 shows the time dependence of the heat release at different temperatures T1 and using Eq. 17 with tTA = 103 s. As expected, at t P tTA the introduction of an additional constant relaxation rate does not influence the heat release. At t & tTA the heat release is larger than taking only into account the one-phonon process (Fig. 4.2). At longer times Q_ decreases exponentially with time. This decrease can be easily understood: the energy levels with long (tunneling) relaxation time have been depopulated at t & tTA at a larger rate. Since the total amount of heat released by the TS should be finite a decrease below the standard result (dashed lines in Fig. 4.2) is expected. To take into account the distribution of potential barriers V and a thermally activated rate we will follow the approach used by Tielbürger et al. [11] and transform Eq. 11 in a double integral in the variables D and V using the approximation l = V/E0 and D0 & 2E0 e–l/p: V 1 Zmax Z PV E E _ Q d dV tanh 2 E0 2kB T0 0
0
tanh
E 1
T0 exp
t=
T0 : 2kB T1
18
For the following discussion it is not relevant to introduce in Eq. 18 a specific distribution of potential barriers V [11]. This is done below for comparison with experimental results and for computing the acoustic properties. After finding the range of potential barriers relevant for the heat release we divided the calculations in two regions: T1 ^ 1 K and T1 > 1 K as described below. In order to find the range of potential barriers relevant for the heat release in our measuring time and temperature ranges we have calculated it following Eq. 18, splitting the Vlimits of the inner integral from Vmin = Vmax – 10 K to Vmax, using only the one-phonon process, and measuring temperature T0 = 0.200 K. We have recognized that for V < 130 K and 52
4.2
Phenomenological theory for the heat release
at t & 103 s the TS are mostly relaxed and do not contribute appreciably to the heat release in our measured time range (104 s ^ t ^ 106 s) any more. The TS that relax through the one-phonon process and are relevant to the heat release are found to be those with potential barriers 130 K < V < 200 K. The contribution of tunneling systems with V > 200 K to the heat release is negligible. At T1 < 1 K the contribution of a thermally activated rate for TS with potential barriers 130 K < V < 200 K is irrelevant, i. e. using t & 10–13 s (from acoustic measurements, see below) we obtain a tTA(V = 130 K kB) of several years. The potential barriers which are relevant in our time and temperature range through a thermally activated rate are V/kB < 10 K, e. g. V (102 s (106 s))/kB & 7 (9) K. We note, however, that according to our calculations TS with those potential barriers already relax at the beginning of the measurement through the one-phonon process. Therefore, at T1 < 1 K we do not expect that thermally activated relaxation influences appreciably the heat release. Our calculations show that thermally activated processes can indeed influence the heat release by depopulating some of the relevant states (100 K ^ V/kB ^ 200 K) during the cooling process if T1 > 1 K. Figure 4.5 shows the calculated heat release as a function of T1 at a given time t = 1.56105 s taking into account the cooling process and one-phonon process as well as thermally activated relaxation rate. The numerical results (Fig. 4.5) show clearly a saturation of Q_ for T1 > 5 K, i. e. at lower temperatures in comparison with the results without thermally activated relaxation, in qualitative agreement with the results assuming Raman processes and experimental results [2]. It is also interesting to note that a thermally activated relaxation rate decreases slightly the exponent in the time dependence of the heat release, i. e. Q_ ! t –a with a < 1. This result is shown in Section 4.4.
Figure 4.5: Heat release at t = 1.56105 s as a function of charging temperature T1 calculated with and without thermally activated processes and a finite cooling rate.
53
4
4.3
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
Experimental details
The experimental setup for measuring the heat release and the specific heat consists of a calorimeter on which the sample is mounted. The samples were cooled from 80 K to 0.050 K in about (5–8)6103 s. The calorimeter is attached to a holder through a thermal resistance or a superconducting heat switch made of an Al strip. The holder is screwed to the mixing chamber of a top loading dilution refrigerator. Two sample holders were used, one from plastic and a second from Teflon. The first one showed a heat release approximately proportional to t –1 whereas for the second one no heat release was measured in agreement with previous measurements [2]. We used two different methods to measure the heat release. Firstly, after cooling to low temperatures (T & 0.060 K) the heat switch was opened and the time dependence of the sample temperature (warmup rate) was measured till about 0.120 K. Then the sample was cooled again to about 0.050 K before starting another warmup run. The heat release is obtained from the slope of the temperature in the warmup run dT (t)/dt with the knowledge of the specific heat of the sample plus calorimeter C (T), i. e. Q_ = C (T) dT (t)/dt. The measurements were completely automated with a personal computer. The background heat leak was about (0.03–0.50) nW at 0.090 K and at t & 105 s depending on the sample holder and the vibration of the connecting cables. To test the measuring setup and procedure we have produced well-known heat leaks with a electrical heater, fixed to the sample. The second method for measuring the heat release is based as before on the measurement of the time dependence of the sample temperature at constant bath (mixing chamber) temperature. The difference lies on the selection of a fixed thermal resistance Rth between sample and holder that enables the semiadiabatic measurement of the heat release in a time scale larger than the intrinsic thermal relaxation time of the arrangement. Approximately 30 minutes after reaching a constant bath temperature Tb the decrease of the sample temperature Ts with time provides directly the heat release, i. e. Q_ = (Ts – Tb)/Rth(Ts ,Tb). The measurement of the thermal resistance together with the background contribution to the heat release is made in situ after reaching the time-independent minimum temperature. Within experimental error (& 10 %) both methods show the same results. The specific heat of both polymers was measured with the heat pulse technique in semiadiabatic fashion. The thermal conductivity was measured with a top loading 3He refrigerator using the standard procedure. The acoustic properties, sound velocity and attenuation, were measured with the vibrating reed technique [16] in the frequency range (0.2–3) kHz. Both polymers were prepared following standard procedures. The PMMA sample had additionally 10 –2 mol% of tetra-4-tert.butyl-phthalocyamin (dye molecule) because it was used in an early optical hole burning experiment [15]. For the specific heat and heat release measurements the mass and density of the PMMA sample were determined as 11.97 g and 1.15 g/cm3, respectively. We have measured two PS samples prepared from different batches. The densities of these samples were 1.05 g/cm3, and the masses 11.4 g (sample PS1) and 38.0 g (sample PS2). For the thermal conductivity measurements two slices were cut from the bulk samples with length l = 1 cm, width w = 2 mm, and thickness d = 300 mm. For the acoustic measurements the reeds had the geometry l = (0.7–1) cm, w = (0.1–0.3) cm and d = (100–300) mm. 54
4.4
4.4
Experimental results and discussion
Experimental results and discussion
4.4.1 Specific heat and thermal conductivity Figure 4.6 shows for both polymers the specific heat devided by the temperature as a square function of temperature. These measurements were performed only when the heat release is negligible (t & 106 s). For t ? ? the specific heat can be written in terms of two contributions: c (T) = c1T + c3T 3 with coefficients for the tunneling system c1 and phonon contribution c3. From Fig. 4.6 we obtain the values c1 = (3.0 + 0.3) mJ/gK2 and c3 = (93 + 18) mJ/gK4 for PMMA, and c1 = (4.6 + 0.5) mJ/gK2 and c3 = (77 + 23) mJ/gK4 for PS. The values of the linear term are in fair agreement with those published by Stephens [17, 18] c1 = 4.6 mJ/gK2 for PMMA and c1 = 5.1 mJ/gK2 for [PS], but we obtained larger phonon contribution (Stephens: c3 = 29 mJ/gK4 for PMMA and c3 = 45 mJ/gK4 for PS). In Figs. 4.7 and 4.8 we compare our specific heat results with data from Ref. [18]. Within the scatter of the data it is difficult to conclude whether the c values are really different.
Figure 4.6: Specific heat divided by the temperature as function of the squared temperature for PMMA (a) and PS (b).
Figure 4.7: Comparison of our specific heat for PMMA with data from Ref. [18].
55
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
Figure 4.8: Comparison of our specific heat for PS with data from Ref. [18].
According to the tunneling model and for t ? ? the specific heat due to the TS is given by [5]: c
T
p2 2 2 k PV ln
T c1 T : umin 6 B
19
If we assume (from heat release data, see below) umin = 10 –10 for PMMA and umin = 6610 –9 for PS and from the measured c1 we obtain a density of states P = 4.061038 (7.561038) 1/Jg for PMMA (PS) in reasonable agreement with the values obtained in earlier specific heat measurements [17] and also from acoustic measurements for PMMA [24]. Recent optical hole burning experiments on PMMA and PS [15] indicate that the density of states of TS for PS is about two times larger than for PMMA in reasonable agreement with our specific heat measurements.
Figure 4.9: Thermal conductivity as a function of temperature for PMMA and PS.
56
4.4
Experimental results and discussion
Figure 4.9 shows the thermal conductivity for PMMA and PS as a function of temperature. For PMMA and at T < 0.7 K we obtain k = 28T 1.84610–3 W/mK2.84 and for PS k = 19T 1.93610 –3 W/mK2.93, in agreement with earlier measurements [17, 19–22], (Figs. 4.10 and 4.11), and with measurements in epoxies [23]. According to the tunneling model and for T < 1 K the thermal conductivity is given by:
T
k3B v 2 1 2
P T ; 6p2
20
where v is the sound velocity and r the mass density. From Eq. 20 and with the sound velo 2 = 9.26105 J/m3 (11.56105 J/m3) for PMMA (PS). If we city from Ref. [17] we obtain Pg replace the density of states P from the specific heat results we obtain similar values for the coupling constant between TS and phonons in both materials g = 0.28 eV (0.27 eV) for PMMA (PS). The results for the thermal conductivity indicate that the density of states of TS for the PS sample is about a factor of two larger than for the PMMA sample.
Figure 4.10: Comparison of our thermal conductivity data for PMMA with earlier publications. The dashed line has been calculated within the tunneling model with parameters taken from our internal friction data.
Figure 4.11: Comparison of our thermal conductivity data for PS with earlier publications. The dashed line has been calculated within the tunneling model with parameters taken from our internal friction data.
57
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
4.4.2 Internal friction and sound velocity Figures 4.12 and 4.13 show the internal friction of PMMA and PS. Below 1 K the internal friction of PMMA and PS is approximately temperature-independent. According to the tunneling model the sound absorption should be temperature-independent in the region otp P 1 (fulfilled in our temperature range) where o = 2 pv is the phonon frequency and tp the relaxation time of the TS (Eq. 6). In this temperature range a simple relationship is found for the internal friction [11, 16] Q
1
p C 2
21
Figure 4.12: Squares: PMMA internal friction as a function of temperature at a frequency of 535 Hz. Full circles: indicate the attenuation data taken from the ultrasonic measurements at 15 MHz from Ref. [24]. Solid and dotted lines: the calculated values for v = 535 Hz and v = 15 MHz following the modified tunneling model considering a thermally activated relaxation rate. For more details see text.
Figure 4.13: Squares and Circles: PS internal friction as a function of temperature at two different frequencies. Solid line: the calculated values for v = 0.24 kHz following the modified tunneling model described in the text.
58
4.4
Experimental results and discussion
2/ru2 and the sound velocity u. Equation 21 should hold even if with the constant C = Pg higher-order processes dominate the relaxation of the TS (if the relaxation rate is proportional to u2 ! D20, Eq. 6). From the temperature-independent value of the internal friction and assuming no background contribution (e. g. due to the clampling) we obtain for PMMA (PS) C % 2.6610–4 (8.3610 –4). Taking into account the mass density, sound velocity, and the coupling constant obtained from the thermal conductivity and specific heat results described above, the values for the parameters C from the internal friction indicate that the density of states of TS for PS is larger than for PMMA by a factor & 2.5. This is slightly larger than that obtained from the specific heat (about 1.5). This might be attributed to the unknown clamping contribution to the measured attenuation (which is always present) or to different umin values (Eq. 19). In Figs. 4.10 and 4.11 we show the calculated thermal conduc 2 values from our internal friction at the plateau. Excellent agreetivity using Eq. 20 with Pg ment is obtained for PMMA (Fig. 4.10) but for PS the thermal conductivity is by a factor of two smaller. This difference might be attributed partially to the background contribution which is not subtracted from the measurement before computing the parameter C. The behaviour of the internal friction above about 3 K is qualitatively different for both polymers. PMMA shows a decrease in the internal friction reaching a minimum at about 30 K and increasing monotonously to the highest temperature of our experiment, 120 K (not shown in Fig. 4.12) in very good agreement with previous work at similar frequencies [25]. On the contrary, the internal friction of PS shows the typical temperature dependence measured for other amorphous materials, for example SiO2 [16]. It increases, reaching a frequency-dependent maximum at T & 37 K (;40 K), (Fig. 4.13), and increases again at T > 60 K (70 K) at the frequency 0.24 kHz (3.2 kHz). This internal friction increase at T > 60 K for PS together with the increase at T > 30 K for PMMA will not be discussed here. Instead, we will discuss the behaviour of the internal friction at lower temperatures in terms of an extension of the tunneling model following the procedure described in Ref. [11]. We assume the simplified relation for a thermally activated relaxation rate given by Eq. 16 and add it to the tunneling rate (Eq. 17). For two well-defined harmonic potentials and within the approximations given by Eq. 10 and with l = V/E0, it can be shown that the internal friction increases linear with temperature just above the temperature-independent region (plateau) [11]: Q
1
pCkB T : E0
22
This increase is observed for PS, (Fig. 4.13); applying Eq. 22 to the results below 20 K we obtain a zero point energy E0 = 13 + 2 K. In the same temperature region and due to the influence of the thermally activated relaxation the relative change of the sound velocity can be written as [11]: uu CkB T ln
!0 : u E0
23
A nearly linear temperature dependence of uu/u is observed in both polymers at temperatures about below 50 K (Figs. 4.14 and 4.15). At T ~ 1 K a crossover, due to tunneling and due to thermally activated relaxation, from the linear T-dependence to the logarithmic 59
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
Figure 4.14: Relative change of sound velocity at v = 535 Hz for PMMA. The solid line represents the linear temperature dependence of the sound velocity at temperatures below 20 K used for the numerical calculations. Inset: the same data but below 10 K in a semilogarithmic scale.
Figure 4.15: Relative change of sound velocity at two different frequencies for PS. The solid line was calculated according to the modified tunneling model described in the text. Inset: the same data but below 10 K in a semilogarithmic scale.
T-dependence can be observed for both polymers (insets in Figs. 4.14 and 4.15). Although the tunneling model with the assumption of thermally activated relaxation of the TS provides a reasonable fit for the linear temperature dependence, its origin is still controversial. We note that a linear temperature dependence of the sound velocity above a few Kelvin is a rather general behaviour observed in several amorphous [26, 27], disordered [28], and polycrystalline metals [29]. Nava [28] argued recently against an interpretation in terms of thermally activated relaxation of the TS for the linear T-dependence of the sound velocity. However, new acoustical results in polycrystalline materials indicate a linear T-dependence of the sound velocity comparable with those found in amorphous materials [29]. Applying Eq. 23 to the measurements at the two phonon frequencies for PS and with the value of E0 from the internal friction we obtain t0 % (1 + 0.5)610 –17 s. As discussed in Ref. [11] the meaning of the prefactor t0 is still unknown. The very small value of t0 found for PS in comparison with the one for SiO2 (t0 % 10 –13 s) should be taken as an ef60
4.4
Experimental results and discussion
fective value until a systematic comparison of the applied model to other experimental data is available. To obtain a maximum in the internal friction an upper limit of the potential height must be assumed. Instead of a cut-off in the distribution P (D, V) and following Ref. [11], a Gaussian distribution with a width s0 will be assumed: P
; V
P
e E0
V 2 =202
:
24
Figures 4.13 and 4.15 show the result of numerical calculations with only the width of the distribution s as free parameter. The fits were obtained assuming s0 = 1200 K and with the values C = 8.3610 –4, v = 0.24 kHz, t0 = 10–17 s and E0 = 13 K using the equations given in Ref. [11]. A reasonable agreement with the experimental data is achieved for both acoustic properties in the expected temperature region. The minimum obtained numerically at T ~ 3 K (Fig. 4.13) has been discussed in Ref. [11] and is attributed to the difference in the number of TS contributing to the relaxation process in the tunneling or thermally activated regime. As pointed out above, the internal friction of PMMA behaves differently from PS above the plateau. It decreases at T > 3 K and reaches a minimum at T ~ 30 K. The predicted linear temperature dependence of the internal friction (Eq. 22), at the measured frequency (v = 535 Hz) is not observed for PMMA. It is tempting to interpret the decrease of the internal friction results above 3 K assuming an upper bound of the TS density of states around 15 K. This assumption has been indeed used to interpret the irreversible line broadening of the optical hole burning experiments [30]. However, ultrasonic attenuation measurements at 15 MHz for PMMA [24] show clearly a thermally activated maximum at 12 K. Therefore we have decided to search for a set of parameters that might explain the low and high frequency results under the assumptions described above and as done for PS. From the sound velocity data below 20 K (Fig. 4.14) and assuming the validity of Eq. 23 (ot P 1) we obtain (E0 /kB) / ln (ot0) % C/(u ln (u)/uT) ~ 0.9 + 0.2. If we assume t0 ~ 10 –17 s like PS, we obtain E0 /kB ~ 30 K. With this value we are not able to obtain a reasonable set of parameters that explain the data. If we take the value for SiO2 from Ref. [11], t0 % 10–13 s, we obtain E0 /kB % (20 + 5) K, a value comparable to that for SiO2. After several trials, eventually we have found a set of parameters that fits reasonably the low and high frequency measurements without the assumption of an energy cut-off. In Fig. 4.12 we compare the experimental results of the internal friction with the numerical calculations for frequencies at 535 Hz and at 15 MHz using E0/kB = 10 K, t0 = 10 –13 s, and a rather small distribution width s0 = 150 K. The model reproduces fairly well the position of the maximum in the attenuation at 15 MHz as well as its relative value in comparison with the plateau [24]. It is worth pointing out, that for PMMA, since the changes produced by the free parameters E0, t0 and s0 compete with each other, it is not possible to find another set of values which can explain the results as well as we can. It is important to note that the internal friction data for both polymers indicate a much smaller thermally activated contribution to the phonon attenuation for PMMA than for PS, in spite of the fact that in the quantum tunneling regime both samples show similar results. This difference may influence the low-temperature heat release because the number of excited states that are available after the cooling process will be different. 61
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
4.4.3 Heat release Figure 4.16 shows the heat release as a function of time for the 12 g PMMA sample at T = 0.090 K and after cooling from 80 K. The heat release follows very well the predicted t –1 law from the tunneling model (Eq. 12). The same result was obtained in different runs with slightly different cooling rates and measuring temperatures 0.070 K ^ T0 ^ 0.110 K. For finite cooling rates and for charging temperatures T1 p 1 K this independence cooling rate is to be expected (Section 4.2.3). As discussed in Section 4.2 the unknown higher-order relaxation processes are taken into account through an effective charging temperature T1. With the tunneling systems density of states from the specific heat and using Eq. 12 we obtain T1 % 26 K. As stated in Section 4.2 for charging temperatures T > 10 K it is not possible to obtain reliable values of the density of states for TS from heat release measurements. From the observed t –1-dependence and using the value for the coupling constant between TS and phonons from Ref. [24], Ak3B = 1.66109 K–3 s –1, we obtain an upper limit for the parameter umin < 10 –10. According to theory, described above, larger values of umin should influence the t –1-dependence in our measuring time scale. From the theoretical results, discussed above, and for a finite cooling rate, thermally activated relaxation (Eq. 16) should influence the absolute value of the heat release, but only slightly its time dependence in our time and temperature ranges. In Figure 4.16 we show the results of the numerical calculations with and without thermally activated processes for a charging temperature T1 = 80 K and using the parameters obtained from the acoustical data (umin = 10 –10). We note that the experimental data lie between the two computed curves (2)
Figure 4.16: Heat release as a function of time. (.): PMMA at measuring temperature T0 = 0.090 K and cooling from T1 = 80 K; (_): Polystyrene (sample PS1) with T0 = 0.090 K and T1 = 80 K, (y): (sample PS2) with T0 = 0.300 K and T1 = 80 K. For PS the curves (1), (3), and (4) are calculated according to the tunneling model with finite cooling rate using the parameters from the fits to the acoustic data. For PMMA the curves (2) and (5) are calculated. In curves (1) and (2) no thermally activated processes are taken into account but for (3), (4) and (5). The parameter umin = 10 –10 with exception of curve (4) where umin = 6610 –9 has been chosen.
62
4.4
Experimental results and discussion
and (5). Even worse, the computed curve (5) with thermal activation shows much smaller values for the heat release by almost two orders of magnitude. This result indicates that too many energy states were depopulated during the cooling process through thermal activation. This disagreement might be ascribed to the assumed potential distribution function (Eq. 24) or the approximation l = V/E0. Curve (2), which is calculated without thermally activated relaxation, lies only a factor of two higher than the measured one (Fig. 4.16) and is in qualitative agreement with the acoustical data where no influence from thermal activation were taken into account. For PS, according to the specific heat and acoustical data (at T < 3 K) and due to a larger density of states of tunneling systems, we expected a larger heat release than for PMMA. Surprisingly, the opposite is observed. After cooling from 80 K with the same cooling rate, the heat release for PS measured at the same temperature as before was at least of a factor of ten smaller than for PMMA (Figure 4.16), and it does not follow the t –1-dependence. In order to understand the observed deviations we have measured the heat release of PS at lower charging temperatures. Figure 4.17 shows the heat release as a function of time at charging temperatures 0.5 K ^ T1 ^ 1 K. The heat release follows very well the t –1-dependence as well as an increase with T21 (Eq. 12, Fig. 4.18). It is interesting to note that a fair quantitative agreement with the prediction of the tunneling model is obtained. If we calculate the density of states of tunneling systems P from these data with Eq. 12 (straight line in Fig. 4.18) we obtain P = 9.0610–38 J–1 g –1 which is similar to the one obtained from the specific heat assuming umin = 6610–9.
Figure 4.17: Heat release as a function of time (in hours) for Polystyrene at a measuring temperature T0 = 0.200 K cooling from different T1. The straight lines have a t –1-dependence.
At higher temperatures T1 we observe the expected saturation of the heat release (Fig. 4.18), however, no deviation from the t –1-dependence has been measured within experimental error. Deviations are observed if we charge the sample at temperatures T1 > 15 K (Fig. 4.16). In this case we have cooled the sample from 80 K and measured the heat release at 0.090 K (sample PS1) and 0.300 K (sample PS2). According to theoretical estimates the observed difference in the heat release between the two PS samples is not attributed to the difference in measuring temperatures. The rather abrupt saturation of the heat release at T1 6 7 K is attributed to the depopulation of the excited states through thermally activated relaxation in the cooling process (Figs. 4.5 and 4.18), as it will become clear below. 63
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
Figure 4.18: Heat release multiplied by the time t as a function of the difference between the squares of charging temperature T1 and measuring temperature T0 for PS. The solid line follows the theoretical prediction with a density of states of tunneling systems 1.45 larger than the one obtained from the specific heat results.
The following experiment provides further verification that the non-simple time dependence of the heat release for PS is due to energy states excited above 15 K and depopulation during the cooling process, very likely through thermally activated relaxation. We have charged the sample at 80 K for several hours and cooled it then to 1 K. We have left the sample for 22 h at 1 K and later continued to 0.3 K, the temperature at which the heat release was measured (Curve (1) in Fig. 4.19). We observe now a clear deviation from the t –1 law. That means that even after 22 h at 1 K the energy states excited above 15 K have not relaxed completely. After 60 h at 0.3 K we warmed the sample to 1 K for 17 h, cooled it to 0.3 K and measured the heat release (Curve (2) in Fig. 4.19). The heat release follows the theoretical t –1-dependence very well. We have calculated the heat release taking one-phonon,thermally activated processes, and the experimental cooling process into account. We used the same parameters obtained from the fit to the acoustical data (Figs. 4.13 and 4.15). With only one free parameter, umin,
Figure 4.19: Heat release as a function of time for PS. (1): cooled from 80 K to 1 K and leaving the sample 17 h at this temperature, T0 = 0.300 K. (2): the sample was warmed to a charging temperature T1 = 1 K for 22 h and cooled again to T0 = 0.300 K. The solid line in (1) is only a guide and the solid line (2) has a t –1-dependence.
64
4.5 Conclusions we can reproduce the measured heat release of PS reasonably well (Fig. 4.16). In this figure we present the two curves (3) and (4) using the parameter umin = 10–10 and 6610 –9. This fit indicates that we can observe the influence of a finite umin through the steeper decrease of the heat release at long times. Curve (1) in Fig. 4.16 was calculated with parameters for PS but without thermally activated relaxation.
4.5
Conclusions
We conclude that thermal conductivity, specific heat and acoustical properties at low temperatures (T < 1 K) can be quantitatively interpreted within the tunneling model for PMMA and PS. At higher temperatures we have measured very different temperature dependence of the internal friction for the two polymers. At the used frequencies and at 0.1 K ^ T ^ 120 K PMMA shows no thermally activated dissipation peak. PMMA shows a minimum in the internal friction at T ~ 30 K where PS shows a maximum. Nevertheless, within the tunneling model and introducing a thermally activated relaxation rate as well as a Gaussian distributon density of states of tunneling systems, it is possible to understand the acoustical properties. From the fits we may conclude that the density of states of tunneling systems for PMMA is restricted to smaller energies, i. e. a smaller width s0, than for PS. Although the thermal conductivity, specific heat, and sound velocity temperature dependence for both samples are similar, the heat release shows different time dependences as well as different values in apparent contradiction with the other measured low-temperature properties. Taking into account the internal friction results, it is tempting to correlate the differences in the heat release between both samples to the difference in the contribution of thermally activated processes in the relaxation of the tunneling states during the cooling process. We have demonstrated that the deviations of the time dependence of the heat release from the t –1-dependence predicted by the tunneling model is due to the relaxation of energy states excited above 15 K. The smaller values of the measured heat release of PS in comparison with the standard tunneling model can be explained by the depopulation of energy states relaxing mainly by thermally activated processes during the cooling process. Without detailed knowledge of the short relaxation times at T1 > 1 K, a quantitative fit or even a qualitative understanding of the heat release Q_ (T1,T0, t) data for high charging temperatures seems to be impossible. Therefore, the heat release with high charging temperatures can be hardly used to obtain information on the density of states of tunneling systems. Heat release experiments at high measuring temperatures T0 > 1 K are necessary to obtain information on the dynamics of the tunneling systems with a relaxation rate not given by the tunneling one-phonon process. These experiments may clarify the influence of the two different relaxation mechanisms discussed nowadays in the literature to interpret the low-temperature properties of amorphous solids above 1 K, namely incoherent tunneling 65
4
Low-Temperature Heat Release, Sound Velocity and Attenuation, …
[31] and thermal activation within the soft potential model [8]. Both approaches have been used with impressive success in the last years. It is, however, not yet clear if incoherent tunneling, a mixture of the two processes (incoherent and thermal activation), or only thermal activation is the main relaxation mechanism of the TS above 1 K.
Acknowledgements
We wish to acknowledge W. Joy for the sample preparation, and S. Hunklinger, D. Haarer and J. Friedrich for valuable discussions. This work was supported by the Deutsche Forschungsgemeinschaft through the Sonderforschungsbereich 213. A. Nittke was supported by the “Graduiertenkolleg Po 88/13” of the Deutsche Forschungsgemeinschaft.
References
1. 2. 3. 4. 5. 6. 7. 8. 9. 10.
11. 12. 13. 14. 15. 16. 17. 18.
66
J. Zimmerman, G. Weber: Phys. Rev. Lett., 46, 661 (1981) M. Schwark, F. Pobell, M. Kubota, R.M. Mueller: J. Low Temp. Phys., 58, 171 (1985) S. Sahling, A. Sahling, M. Kolac: Solid State Commun., 65, 1031 (1988) P.W. Anderson, B.I. Halperin, C.M. Varma: Phil. Mag., 25, 1 (1972); W.A. Phillips, J. Low Temp. Physics 7, 351 (1972) M. Deye, P. Esquinazi: Z. Phys. B – Condensed Matter 76, 283 (1989) M. Deye, P. Esquinazi: in: S. Hunklinger, W. Ludwig, G. Weiss (eds.): Phonon 89, World Scientific, Singapore, p. 468, (1990) J. Jäckle: Z. Phys., 257, 212 (1972) D. Parshin, S. Sahling: Phys. Rev. B, 47, 5677 (1993) J.J. Brey, A. Prados: Phys. Rev. B, 43, 8350 (1991) P. Esquinazi, M. Scherl, Li Junyun, F. Pobell: in: M. Meissner, R. Pohl (eds): 4th International Conference on Phonon Scattering in Condensed Matter, Springer Series in Solid State Sciences, Vol. 112, p. 287 (1993) D. Tielbürger, R. Merz, R. Ehrenfels, S. Hunklinger: Phys. Rev. B, 45, 2750 (1992) P. Doussineau, C. Frenois, R. G. Leisure, A. Levelut, J. Y. Prieur: J. Phys. (Paris), 41, 1193 (1980) S. Hunklinger, W. Arnold: in: W. P. Mason, R. N. Thurston (eds.): Physical Acoustics, Vol XII, Academic Press, New York, 1976 W.A. Phillips: in: S. Hunklinger, W. Ludwig, G. Weiss (eds.): Phonon 89, World Scientific, Singapore, p. 367 (1990) K.-P. Müller, D. Haarer: Phys. Rev. Lett., 66, 2344 (1991) A.K. Raychaudhuri, S. Hunklinger: Z. Phys. B – Condensed Matter, 57, 113 (1984) R.B. Stephens: Phys. Rev. B, 8, 2896 (1973) R.B. Stephens, G.S. Cieloszyk, G.L. Salinger: Physics Letters, 28A, 215 (1972)
References 19. 20. 21. 22. 23. 24.
25. 26. 27. 28. 29. 30. 31.
D. Cahill, R. Pohel: Phys. Rev. B, 35, 4067 (1987) C. Choy, G. Salinger, Y. Chiang: J. of Applied Physics, 41, 597 (1970) J. Freeman, A. C. Anderson: Phys. Rev. B, 34, 5684 (1986) J. Mack, J. Freeman, A.C. Anderson: J. of Non Crystalline Solids, 91, 391 (1987) G. Hartwig: Progr. Colloid and Polymer Sci., 64, 56 (1978) G. Federle, S. Hunklinger: J. de Physique, C9(12), Tome 43, p. C9–505 (1982); G. Federle: PhD Thesis, M. Planck Stuttgart, 1983, unpublished; A.K. Raychaudhuri: in: T.V. Ramakrishnan, M. Raj Lakshmi (eds.): Non-Debye Relaxation in Condensed Matter, World Scientific, p. 193 (1987) J. Crissman, J. Sauer, E. Woodward: J. of Polymer Science, A2, 5075 (1964) G. Bellesa: Phys. Rev. Lett., 40, 1456 (1978) J.-Y. Duquesne, G. Bellesa: J. de Physique Lettres, 40, L-193 (1979) R. Nava, R. Oentrich: J. of Alloys and Compounds, in press; R. Nava, Phys. Rev. B, 49, 4295 (1994) E. Gagemidze, P. Esquinazi, R. König: Europhys. Letters, 31, 13 (1995) W. Köhler, J. Zollfrank, J. Friedrich: Phys. Rev. B, 39, 5414 (1989) A. Würger: in: From coherent tunneling to relaxation, Springer Tracts in Modern Physics, Vol. 135, (1997)
67
5
Spectral Diffusion due to Tunneling Processes at very low Temperatures Hans Maier, Karl-Peter Müller, Siegbert Jahn, and Dietrich Haarer
5.1
Introduction
Pioneered by the work of Zeller and Pohl [1] it was discovered in the early 1970s that amorphous solids show low-temperature thermal and acoustic properties which are very different from those observed in crystals. For reviews see for example Refs. [2, 3]. The most wellknown of these anomalous properties is the specific heat, which is in general considerably larger than would be expected from the Debye model and varies linear with temperature in contrast to the Debye T3-dependence. Other anomalies are the temperature dependence of the thermal conductivity, the properties of phonon echoes, and ultrasonic absorption. These features seem to be quite universal for all kinds of amorphous solids, irrespective of their chemical composition and structure, i. e. inorganic as well as organic or polymeric. Very soon after the first experimental evidence for these anomalous low-temperature excitations Anderson et al. [4] and independently Phillips [5] developed a theoretical description, called the tunneling model [4, 5]. It is based on the assumption that the low energy degrees of freedom in amorphous solids arise from tunneling motions of atoms or groups of atoms between local energetic minima which should exist in any disordered solid. If only the lowest energy level of each minimum is considered, this leads to two eigenstates. For this reason, these degrees of freedom are often referred to as two-level system (TLS). An important consequence of this model is the formal analogy to a system of particles with spin 1/2, which for example immediately explains the existence of phonon echoes. Another very striking feature of the tunneling model was the prediction of a time-dependent specific heat [4]. This was confirmed experimentally several years later [6]. Furthermore, the model can explain the heat release [7] of amorphous solids, which is a time-dependent non-equilibrium phenomenon. From these kinds of experiments, it could be concluded that TLS dynamics occur on time scales extending over many orders of magnitude. The sensitivity of optical experiments on amorphous solids was hindered, in many instances, by the large inhomogeneous broadening which arises from the distribution of local environments of the involved optical transitions. Therefore a very important step was the discovery of persistent spectral hole burning in 1974 [8, 9]. This method of high-resolution laser spectroscopy eliminates the inhomogeneous effects induced by the static disorder in 68
Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
5.2
The optical cryostat
amorphous hosts. For this purpose dye molecules are embedded in the solid which change their absorption spectra when irradiated with resonant narrow band laser light. This produces a dip in the inhomogeneous absorption band, called a spectral hole. A narrow spectral hole can be regarded as a highly sensitive spectral probe for any kind of distortion of the matrix, which induces small spectral changes [10]. In this way variations of strain fields caused by pressure changes of almost some 10 hPa can be detected [11]. Spectral holes are also sensitive to small changes of other external parameters including electric fields [12, 13]. After observing quite a few anomalous properties of optical transitions in glasses and attributing them to the dynamics of TLS [14], the tunneling model was adopted by Reinecke [15] to explain the low-temperature line widths of optical transitions in amorphous solids using the concept of spectral diffusion. This concept had originally been developed for the description of spin resonance experiments [16] and had already been applied to the theoretical treatment of the above mentioned ultrasonic properties of glasses [17]. Soon after this step, the possibility of a connection between thermal and optical properties of amorphous solids was supported by the observation of time dependence of spectral hole widths [18]. The application of the tunneling model to the description of spectroscopic properties proposed an important link suggesting a correlation between the specific heat and the optical line width. This implies that, besides the mentioned calorimetric and acoustic methods, optical spectroscopy yields information about the dynamics of the same low energy excitations of amorphous solids, which dominates the calorimetric experiments. A crucial point in establishing this connection is the temperature dependence of these physical solid state parameters. The tunneling model in its original form predicts linear temperature dependence for the specific heat as well as for the optical line width. This prediction, however, is only valid at temperatures where the contribution of phonons is of minor importance. Earlier hole burning measurements on the temperature dependence of optical line widths [19] indicated the necessity of expanding the temperature range accessible to optical absorption spectroscopy to values far below 1 Kelvin in order to exclude any other mechanisms except TLS dynamics. For this reason we have constructed a 3He/ 4He dilution refrigerator with optical windows allowing transmission spectroscopy at temperatures down to 0.025 K, a temperature regime in which only very few data from optical spectroscopy existed before [20, 21]. In addition, cooling with a 3He/ 4He mixture can be performed continuously for very long times (in principle unlimited) if the necessary care in cryostat design and operation is taken. In our experiments we have reached operation times up to three months.
5.2
The optical cryostat
In the design of a cryostat for optical spectroscopy two main problems have to be overcome. In an absorption experiment the sample has to dissipate the absorbed energy in order to avoid overheat during the measurement. Therefore the best possible thermal contact to the cold stage is of extreme importance. The second problem is how to guide the laser light to the sample without creating an intolerably large additional heat leak, for example by infrared 69
5
Spectral Diffusion due to Tunneling Processes at very low Temperatures
irradiation from the windows. Since various construction methods for optical cryostats in the temperature range below 0.500 K did not yield the desired results, special care had to be taken in the design of our dilution refrigerator. For example it had been reported [22] that for samples located outside the mixing chamber temperatures below 0.300 K could not be reached, even if the best thermal contact is realized by pressing the samples to the wall of the mixing chamber with indium metal as contact material. In another kind of experiment a glass fibre winding around the cold finger of a dilution refrigerator shows a significant temperature gradient with respect to the mixing chamber below 0.100 K [20]. For these reasons, we decided to place the sample directly into the dilute phase of the mixing chamber. This way optimal thermal contact and a constant temperature of the sample was achieved via the superfluid 4He. For performing optical experiments the mixing chamber was designed as a glass cylinder. The optical path, used in our cryostat, is shown in Figure 5.1 [23]. Three sets of windows are mounted on cold copper shields to eliminate most of the room temperature radiation in three steps: at liquid nitrogen temperature (77 K), liquid helium temperature (4.2 K), and at approximately 1 K, the latter being achieved by cooling with the pumped 3He of the distillation chamber. In contrast to other constructions, the vessel containing the dilution refrigerator part of the cryostat is in our design not surrounded by the helium tank which has the advantage that the laser beam is not scattered by boiling liquid helium. We estimate that the total heat leak caused by room temperature radiation is below 50 nW. The minimum temperature reached is 0.024 K. The cooling power is about 6 mW at 0.100 K. Although this is a very low value, it is sufficient since the power of the absorbed laser light was always far below 1 mW. The light powers used for hole burning in our experiments were on the order of several nanowatts to several tens of nanowatts depending on the temperature. For hole detection the power is reduced to the picowatt range. The cooling power of our cryostat and the thermal conductivity of the involved polymers are high enough to guarantee a uniform temperature distribution with no significant sample heating during the hole burning process. mixing - chamber He - shield 1-K - shield LN2 - shield sample 4
Figure 5.1: Alignment of optical windows and sample in the cryostat. The sample is placed inside the mixing chamber of the dilution refrigerator. The shields are connected to the distillation chamber, the helium tank, and the nitrogen tank, respectively. The liquid N2 windows possess an infrared reflective coating.
70
5.3
Theoretical considerations
The temperature is measured with a RuO2 thick film resistor (TFR) supplied by Phillips (type RC-01). The heat capacity and thermal relaxation time of the TFR are equivalent to those of a carbon resistor but its thermal reproducibility during temperature cycles is better [24]. The resistor is calibrated against several primary and secondary thermometers including a NBS fixed point device, CMN and Ge, thermometers. Its accuracy is better than 2 % in the temperature range between 4.2 K and 0.025 K. The thermometer is placed into the dilute phase of the mixing chamber in direct thermal contact to the sample. The resistance is measured using a four wire ac resistance bridge (AVS-46 RV Elektroniikka, Finland). At the minimum temperature, the energy dissipated in the resistor is less than 0.5 pW.
5.3
Theoretical considerations
In the tunneling model [4] the TLS was described by two parameters (Fig. 5.2), the asymmetry parameter D and the overlap parameter l, which contains the barrier height, the distance of the two minima, and the mass of the tunneling particle. They are related with the total energy splitting E of the two levels and the tunneling matrix element D0 by the relations E
q 2 20
and
0 k exp
;
1
where kO is a typical zero point energy. One of the most important ingredients of the TLS model is the distribution function characterizing the two parameters. The originally used assumption for this function, which has also been applied to explain spectral diffusion [15, 17], is a flat distribution in both parameters, namely P
; dd Pdd :
2
Figure 5.2: Double minimum potential as a model for a TLS. All relevant parameters are shown in the figure.
71
5
Spectral Diffusion due to Tunneling Processes at very low Temperatures
It is convenient, however, to use experimentally accessible quantities as variables, i. e. the energy E and a dimensionless relaxation rate R, which can be defined as: R = r/rmax = D20 / E2. The transformation to the new variables yields for the distribution function [25]: P
E; R P
1 p : 2R 1 R
3
A very important feature of this distribution is the fact that P (E, R) is independent of E. In order to keep the total number of TLS finite, some cut-off value for R ? 0 has to be introduced [3], which is usually denoted by Rmin . It was shown in Ref. [15] that for optical transitions in glasses the TLS dynamics results in spectral diffusion, which shows up in the experiment as a time and temperature-dependent Lorentzian line broadening. The width of this Lorentzian line must be calculated by averaging over the distribution of energies and relaxation rates P(E, R). It can be written as: 2p2
t; T Cij 3k
E Zmax
Emin
Z1 dEn
T
dR
Rmin
P
E; R
1 E
exp trmax R :
4
Here ACijS represents an average coupling constant between the TLS and the optical transition, n (T) is a thermal occupation factor of the TLS states. For the system which is investigated in this work, the parameter rmax can be estimated from experimental data on ultrasonic attenuation [26] to be on the order of 107 s –1 at a temperature of 0.100 K and even larger at higher temperatures. Therefore, the condition t 7 rmax p 1 is well fulfilled on all time scales exceeding several microseconds. In this limit the rate integration in Eq. 4 can be performed analytically [27], which leads to the well-known logarithmic time dependence of spectral diffusion: !
t; T
p2 Cij P kB T ln
rmax t : 3k
5
Equation 5 represents the theoretical prediction of the tunneling model for the time and temperature-dependent broadening of spectral holes. This result, however, is the result of a particular form of the density of tunneling states P (E, R), which is based on the a priori assumption of Eq. 2. A uniform density of states in D is a physically reasonable choice; the independence of l, however, is difficult to justify, since l consists of several parameters [28]. The temperature dependence of spectral diffusion is dominated by D the time evolution stems mainly from l. Therefore, these two predictions from Eq. 5 do not have the same validity. In our experiments we have investigated time and temperature dependence separately.
72
5.4
5.4
Temperature dependence
Temperature dependence
In these experiments, we investigated polystyrene (PS) doped with phthalocyanine and polymethylmethacrylate (PMMA) doped with tetra-4-tert-butyl phthalocyanine. Both sample materials have also been investigated by heat release and specific heat measurements [29]. The samples had optical densities of about 0.4 at a typical thickness of 3 mm. The samples were prepared by bulk polymerisation of the solution of the dye in the monomer. The observed hole shapes are Lorentzian with no detectable deviations in all cases. To eliminate saturation effects at least 10 holes with different energies were burned at each temperature and the homogeneous line width was determined by extrapolation to zero burning fluence [30]. Due to their low relative depths the extrapolation was done assuming a linear dependence of the hole area on energy [10]. A weak variation of the line width with light power was observed at our minimum temperature of 0.025 K for PMMA. We attribute this variation to sample heating. The temperature dependence of the hole width is shown in Fig. 5.3 [23]. The results are: a) both systems display a linear temperature dependence over the whole temperature range from 0.500 K down to 0.025 K and no crossover to a constant line width is seen. The linearity of the data plot shows that the density of states P (E, R) is indeed independent of the TLS energy; b) the relative magnitude of the line width in the two systems correlates with the respective specific heat [31]; c) the extrapolated line width for T ? 0 is nearly the same for both systems, confirming that in an amorphous system the line width reaches the lifetime limited value Gh = 1/2 pT1 (Heisenberg limit) of the electronic transition only when T ? 0. This limit is reached in our experiment within 10 %!
Figure 5.3: Temperature dependence of the hole burning line width for PS and PMMA between 0.025 K and 0.500 K.
73
5
Spectral Diffusion due to Tunneling Processes at very low Temperatures
In the case of PS, where unsubstituted phthalocyanine was used as dye, the result for the extrapolated line width G (T ? 0) is in very good agreement with the fluorescence lifetime measurements of this molecule [32]. We are not aware of measurements of the fluorescence lifetime of substituted phthalocyanine, but our results show that there is no major difference between both dyes as far as their excited state lifetimes are concerned. These results imply that in amorphous solids there are dynamical processes of twolevel systems with an energy spectrum extending down to values as low as kB 7 0.025 K. These low-energy excitations dominate the line widths of optical transitions even at low temperatures and the lifetime limited value can only be reached by extrapolating to zero temperature.
5.5
Time dependence
After the system has been cooled down spectral holes are burned immediately and after some delay times, while the sample was at constant temperature, we observe a hole broadening which depends on this delay time. This behaviour is demonstrated in Fig. 5.4. Dataset A is the broadening of a hole which is burned immediately after the sample (phthalocyanine in PMMA) has been cooled from liquid nitrogen temperature to 0.300 K. The curves show the evolution of holes burned about one day, three days, and one week after cooling down. The amount of spectral diffusion in a given time interval decreases continuously until a small residual effect becomes observable, which is independent of the time delay after reaching the final temperature. This is represented by dataset B in Fig. 5.4.
A
B
Figure 5.4: Time evolution of spectral holes burned at different times after sample cooling. Datasets corresponding to A and B are investigated in the following.
74
5.5
Time dependence
Investigating the temperature dependence of the time evolution of the hole width [33], we performed experiments on a PMMA sample doped with phthalocyanine at different temperatures T, varying from 0.100 K to 1 K. For each of the temperatures T = 0.100, 0.300, 0.500, and 0.700 K, the respective experiments were carried out in a separate run. It took about one hour to cool the system from 77 K to 4 K. The time for cooling down from 4 K to the final temperature T depends slightly on T, but is in the range of about (6 + 1) hours. Immediately after reaching T, holes are burned and their subsequent broadening is observed for about one week. These experiments yield data corresponding to set A in Fig. 5.4. The results of these measurements are shown in Fig. 5.5 [33]. In this plot the time origin for each run is identical, namely the time at which the cooling down procedure from 77 K was started. For better visibility, however, the data corresponding to T = 0.500, 0.300, and 0.100 K are shifted by 0.5, 1.0, and 1.5 orders of magnitude along the logarithmic time axis, respectively. Except for the data taken at 0.500 K the total observation time was 6–10 days.
Figure 5.5: Broadening of holes burned immediately after reaching T. Data shifted for better visibility (see text).
Keeping the samples at constant temperature new holes are burned after 1–2 weeks and their broadening is observed for several hours, corresponding to set B in Fig. 5.4. These data are shown in Fig. 5.6 [33]. Here the observation time is 2–16 hours. Note that the range of the DG-axis is about 10 times less as compared with Fig. 5.5. Comparing our data of Figs. 5.5 and 5.6, it is obvious that the measurements which are started immediately after cooling down show no variation of the observed broadening with the phonon bath temperature, while the residual behaviour observed many days later exhibits a rather pronounced dependence on the experimental temperature. It has to be emphasized that the data shown in Fig. 5.5 and the corresponding data in Fig. 5.6 for the same values of T were measured without any change of temperature in between the two subsequent experiments. In spite of the variation of the final temperature over almost one order of magnitude, all four datasets in Fig. 5.5 show the same hole broadening behaviour. We attribute this to the existence of a non-equilibrium state of the TLS ensemble due to the fast cooling procedure: The large amount of spectral diffusion observed after fast 75
5
Spectral Diffusion due to Tunneling Processes at very low Temperatures
Figure 5.6: Broadening of holes burnt after 1–2 weeks at low temperature.
cooling is due to the relaxation of TLS to their thermal equilibrium [34]. This relaxation process is known to produce the thermal phenomenon of heat release [7]. Thus, it can be concluded that we have established an important connection between optical and calorimetric phenomena. The data of Fig. 5.6 exhibit a pronounced dependence on temperature, as can be expected from theoretical considerations outlined in Section 5.3 and from the non-time resolved experiments of Section 5.4. The time evolution, however, shows a distinct non-logarithmic behaviour in contradiction to the prediction of the tunneling model. For short times the Fig. 5.6 shows clearly that the hole broadening starts fairly logarithmic. We have performed transient hole burning experiments on the millisecond time scale, which also yielded a logarithmic behaviour [35]. At longer times, however, the diffusional broadening increases faster than logarithmic. This increase occurs later at lower temperatures, which is to be expected from the temperature dependence of the relaxation rates. These new features are in qualitative agreement with theoretical work that invokes strong coupling of TLS with phonons [28, 36]. We believe that our experimental work shows that the method of spectral hole burning spectroscopy is suitable for studying the low-temperature properties of amorphous solids. Especially for the investigation of the long-time behaviour of TLS equilibrium dynamics, where other methods cease to function, it is a very powerful experimental technique.
References
1. R.C. Zeller, R.O. Pohl: Phys. Rev. B, 4, 2029 (1971) 2. Amorphous Solids. Low Temperature Properties, in:W.A. Phillips (ed.): Topics in current Physics, Vol. 24, Springer, Berlin, (1981)
76
References 3. S. Hunklinger, A. K. Raychaudhuri: in: D. F. Brewer (ed.), Progress in Low Temp. Physics, Vol. IX, Elsevier Science, Amsterdam, p. 265 (1986) 4. P.W. Anderson, B.I. Halperin, C.M. Varma: Philos. Mag., 25, 1 (1972) 5. W.A. Phillips: J. Low Temp. Phys., 7, 351 (1972) 6. M.T. Loponen, R.C. Dynes, V. Narayanamurti, J.P. Garno: Phys. Rev. Lett., 45, 457 (1980) 7. J. Zimmermann, G. Weber: Phys. Rev. Lett., 46, 661 (1981) 8. B.M. Kharlamov, R.I. Personov, L.A. Bykovskaya: Opt. Commun., 12, 191 (1974) 9. A.A. Gorokhovskii, R.K. Kaarli, L.A. Rebane: JETP Lett., 20, 216 (1974) 10. J. Friedrich, D. Haarer: Angew. Chem., 96, 96 (1984); Angew. Chem. Int. Ed. Engl., 23, 113 (1984) 11. Th. Sesselmann, W. Richter, D. Haarer, H. Morawitz: Phys. Rev. B, 36(14), 7601 (1987) 12. A.P. Marchetti, M. Scozzafara, R.H. Young: Chem. Phys. Lett., 51(3), 424 (1977) 13. V.D. Samoilenko, N.V. Rasumova, R.I. Personov: Opt. Spectr., 52(4), 580 (in Russian) (1982) 14. P.M. Selzer, D.L. Huber, D.S. Hamilton, W.M. Yen, M.J. Weber: Phys. Rev. Lett., 36, 813 (1976) 15. T.L. Reinecke: Solid State Commun., 32, 1103 (1979) 16. J.R. Klauder, P.W. Anderson: Phys. Rev., 125(3), 912 (1962) 17. J.L. Black, B. I. Halperin: Phys. Rev. B, 16, 2879 (1977) 18. W. Breinl, J. Friedrich, D. Haarer: J. Chem. Phys., 81(9), 3915 (1984) 19. G. Schulte, W. Grond, D. Haarer, R. Silbey: J. Chem. Phys., 88(1), 679 (1988) 20. M.M. Broer, B. Golding, W.H. Haemmerle, J.R. Simpson, D.L. Huber: Phys. Rev. B, 33, 4160 (1986) 21. A. Gorokhovskii, V. Korrovits, V. Palm, M. Trummal: Chem. Phys. Lett., 125, 355 (1986) 22. Korrovits, M. Trummal: Proceedings of the Academy of Sciences of the Estonian SSR, 35(2), 198 (1986) 23. K.-P. Müller, D. Haarer: Phys. Rev. Lett., 66, 2344 (1991) 24. W.A. Bosch, F. Mathu, H.C. Meijer, R.W. Willekers: Cryogenics, 26, 3 (1985) 25. J. Jäckle: Z. Phys., 257, 212 (1972) 26. G. Federle: PhD thesis, Max-Planck-Institut für Festkörperforschung Stuttgart (1983) 27. S. Hunklinger, M. Schmidt: Z. Phys. B, 54, 93 (1984) 28. K. Kassner: Z. Phys. B, 81, 245 (1990) 29. A. Nittke, M. Scherl, P. Esquinazi, W. Lorenz, Junyun Li, F. Pobell: J. Low Temp. Phys., 98(5/6), 517 (1995) 30. L. Kador, G. Schulte, D. Haarer: J. Phys. Chem., 90, 1264 (1986) 31. K.P. Müller: PhD thesis, Universität Bayreuth (1991) 32. W.H. Chen, K.E. Rieckhoff, E.M. Voigt, L.W. Thewalt: Mol. Phys., 67(6), 1439 (1989) 33. H. Maier, D. Haarer: J. Lum., 64, 87 (1995) 34. S. Jahn, K.-P. Müller, D. Haarer: J. Opt. Soc. Am. B, 9, 925 (1992) 35. S. Jahn, D. Haarer, B.M. Kharlamov: Chem. Phys. Lett., 181, 31 (1991) 36. K. Kassner, R. Silbey: J. Phys. Condens. Matter, 1, 4599 (1989)
77
6
Optically Induced Spectral Diffusion in Polymers Containing Water Molecules: A TLS Model System Klaus Barth, Dietrich Haarer, and Wolfgang Richter
6.1
Introduction
In the past decade much experimental and theoretical work was done on spectral diffusion in amorphous solids. It turned out that at low temperatures, optical dephasing phenomena [1] as well as the numerous caloric data [2] can be well described by assuming the presence of low-energy excitations, the so-called two-level systems (TLS). Photochemical hole burning [3] and optical echo experiments [4] have provided experimental evidence for different dynamics of optical transitions in glassy systems as compared to crystalline matrices. For glassy organic solids the TLS concept was first proposed by Small and co-workers [5, 6] and was later used by Reinecke [7] to explain low-temperature optical line widths. Especially the photochemical hole burning data over long observation periods (observation times longer than three months) at temperatures down to 0.050 K allowed a critical test of the theoretical approach within the tunneling model [8]. Theoretical and experimental results to this topic are also given in this book by H. Maier et al. At temperatures above 1 K tunneling transitions and localized vibrations influence the physical properties [9]. Both types of mechanisms have recently been incorporated in the soft potential model [10] which contains the well-known tunneling model as a special case. A microscopic interpretation of optical line broadening phenomena in terms of e. g. local excitations of the matrix or switching of optically addressed chemical groups suffered from the lack of experimental data. In the past, several experimental techniques have been developed to shed light on the microscopic mechanisms of the phenomena. These techniques are all based on the generation of phonons in the matrix material, especially in the neighbourhood of the spectral probe. Heat pulses from external heaters [11] produce a broad distribution of phonon frequencies inside the chromophore host system and permit the investigation of the dynamics of barrier crossings and the coupling between the TLS and the dye molecules [12]. Light-induced phonon generation in hole burning systems can in principle be achieved either by exciting non-radiative decay processes in appropriate chromophores [13] or by direct absorption of IR light in the matrix material [13, 14]. The non-radiative decay method, which has been used to study transient and irreversible spectral diffusion processes, yields also a broad distribution of phonon frequencies and gives rise to similar experimental processes as e. g. the heat pulse technique. On the other hand, the IR absorption 78
Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
6.2
Experimental setup for burning and detecting spectral holes
method where the sample is illuminated with narrow band IR light allows us to generate phonons of high density and of a comparatively small energy distribution in the direct neighbourhood of the optical probe. The contribution of the broad band black-body background radiation can be minimized by using an appropriate intensity of a narrow band IR source. For the optical investigation of amorphous systems, photochemical hole burning (PHB) is a high-resolution technique and a powerful tool to examine local sites in polymers at low temperatures. Dye molecules embedded in polymers at low concentration exhibit strongly inhomogeneously broadened absorption bands in a conventional spectroscopic experiment. Selecting an ensemble of these dye molecules with narrow band laser light, which gives rise to a photoreaction, leads to a sharp spectral dip at the laser frequency, the so-called spectral hole. Due to the high resolution, this method is appropriate for detecting small perturbations in the matrix such as a transient change of the phonon distribution or permanent matrix rearrangements in the vicinity of the dye molecules. Such rearrangements can be due to a configurational change of parts of the polymer main chain or due to a reorientation of small molecules (water), which may be embedded in the matrix in addition to the dye molecules. In the following, two different experimental conditions are discussed which are based on the absorption of IR light. Both experimental situations lead to a change of the local interaction of the optical probe with its local matrix environment. In the first part the phonons are treated as a time-dependent temperature bath. In the second part experiments are discussed where local groups of the matrix are selectively addressed by IR radiation of very low intensity. The observed enhanced spectral diffusion shows a characteristic dependence on the IR frequency and coincides with only a few of the numerous IR absorption bands. A quantitative description of this new process together with the identification of the resonant vibrations is given within a simple kinetic model.
6.2
Experimental setup for burning and detecting spectral holes
The experimental setup for burning and detecting spectral holes with a narrow band laser is described elsewhere [16]. The experiments were performed at 1.8 K in a bath cryostat in which the sample was immersed in superfluid helium. As samples we used different polymeric matrices such as polymethylmethacrylate (PMMA), polyamide (PA), polyethylene, polystyrene, etc. doped with free base phthalocyanine (H2Pc) at low concentration (10 –2 mol%). Their preparation is described in Ref. [16]. The water content of the samples has been controlled by heating them under vacuum conditions. Because of its strong hydrophilic nature PMMA has a high capacity of water absorption at atmospheric conditions. In order to investigate the influence of the water molecules the experiments, described in Section 6.4, were carried out either with a nearly water-free PMMA sample or with a PMMA sample containing water molecules under equilibrium conditions. The optical windows of the cryostat consisted of crystalline BaF2 which allowed the study of hole burning spectra in the lowest vibrational band of the electronic S0 ? S1 transition of H2Pc at about 0.69 mm as well as under IR illumination between 2 mm and 11 mm. In this setup, the broad band background radiation with an emission 79
6
Optically Induced Spectral Diffusion in Polymers Containing Water Molecules
maximum at 10 mm has an integrated intensity of about 300 mW/cm2 at the location of the sample. As IR radiation sources we used a Globar with a maximum emission intensity near 3 mm and different CO2 laser lines around 10 mm. An acousto-optic modulator was used for reducing the intensity of the CO2 laser down to 1 W/cm2 and for switching with times some microseconds. The radiation of the Globar was dispersed in a monochromator and with different dielectric filters to a bandwidth between 0.05 mm and 0.2 mm with typical intensities around 100 mW/cm2.
6.3
Reversible line broadening phenomena
In this Section the mechanisms of reversible line broadening phenomena under continuous or pulsed irradiation conditions are discussed. Phonons are generated by illuminating the polymeric sample with the light of a single CO2 laser line. The wavelength of the CO2 laser was selected to generate high frequency phonons only within a small penetration depth of less than 10 mm. The dye molecules, which are homogeneously distributed throughout the sample thickness of some 100 mm, are a local probe for the increase in the phonon density during the IR irradiation. Due to the thermalisation processes, phonons show a broad energy distribution. This change of the phonon distribution gives rise to an increased effective temperature under cw irradiation conditions. Because of the high cooling rate of the surrounding superfluid helium, typical irradiation intensities of about 1 W/cm2 were used to obtain a significant increase in the phonon density. The influence on the homogeneous line width of the dye molecules can be investigated in a zero burning fluence experiment, i. e. the limit of the hole width is given by extrapolating to zero burning fluence. The lower curve in Fig. 6.1, which was measured without any IR irradiation, yields an extrapolated value for the line
Figure 6.1: Zero burning fluence experiment under different phonon density conditions in polyamide doped with H2Pc (see text).
80
6.3 Reversible line broadening phenomena width of about 375 MHz. The two upper curves show increased hole widths due to an enhanced phonon generation either by IR irradiation during the burning process only(triangles) or during the detection process only(circles). The profile of a spectral hole can be written as Z1 A
!
!L /
nz
!0
!L z
!
!0 d!0 ;
1
1
where nz (o' – oL) is the site distribution function of the molecular line contributing to the hole spectrum and z (o – o') is the absorption profile of a single molecule. On the time scale of this experiment (up to some minutes) the spectral hole profiles are mainly reversible (see also Fig. 6.2 and Fig. 6.3). Therefore, the homogeneous line profile function z (o) is much more affected by the altered phonon density than the site distribution function nz (o). Thus, it is obvious that the two upper curves in Fig. 6.1 are similar and give for the hole width nearly the same zero burning fluence value of 440 MHz. Both curves are well separated from the lower curve which was obtained without any additional phonon generation. Applying an effective temperature model the difference between these two zero burning fluence values corresponds to a temperature change of about 0.3 K within the sample. Because of the strongly inhomogeneous experimental conditions during phonon generation and phonon diffusion through the sample, however, each different subensemble of dye molecules experiences a different distribution in phonon energies and, as a consequence, a bath description in terms of one single temperature is not appropriate. By using different op-
Figure 6.2: Lower part: Spectral profile of a photochemical hole with and without phonon generation during the detection process. Upper part: Directly measured difference between these two profiles as obtained by modulating the IR light at a frequency of 150 Hz.
81
6
Optically Induced Spectral Diffusion in Polymers Containing Water Molecules
Figure 6.3: Decay of the transmission maximum during a laser pulse.
tical energies for the phonon generation, it is in principle possible to study the contribution of different matrix vibrations on the dephasing of a single absorber function z (o). The time scale of the hole burning experiments discussed above is several minutes. It is about 3 orders of magnitude larger than the typical thermal relaxation time of the sample as given by
d 2 c ;
2
where d is the dimension (thickness) of the sample, c the specific heat, r the mass density, and k the thermal conductivity. For the temperature of our experiment (1.8 K) and a typical sample dimension of 1 mm the thermal relaxation time t is calculated to 10 ms. A consequence of this short relaxation time is shown in Fig. 6.2 and Fig. 6.3. The two spectral holes in the lower part of Fig. 6.2 were obtained with and without phonon generation during the hole detection process. A modulation of the IR light during the detection process results in a continuous switching between these two hole profiles. In the upper part of Fig. 6.2, a modulation frequency of 150 Hz was used during the scan of the optical frequency. The switching time between the two hole profiles is of the same order of magnitude as the thermal relaxation time. The continuous switching between the two hole profiles is detected with lock-in technique. The result shows that the phonon generation and relaxation process is sufficiently fast to follow the 150 Hz modulation of the IR light. A time-resolved experiment is shown in Fig. 6.3. The optical transmission at the peak of a hole spectrum was monitored while the sample was being illuminated with a single CO2 laser pulse of 600 ms duration. The decay of the transmission signal cannot be described with a single exponential function. It is well represented by the superposition of two exponentials with a fast contribution t1 & 10 ms and a slow contribution t2 & 150 ms. The fast contribution is close to the thermal relaxation time at the temperature of the helium bath. The slow contribution contains all the inhomogeneous experimental conditions as mentioned above, in particular a temperature gradient inside the sample that gives rise to a variation of the thermal relaxation time. Since the amplitude of the fast contribution is larger by a factor of 4, the switching time between the two curves in Fig. 6.2 is mainly determined by the fast contribution t1. 82
6.4
Induced spectral diffusion
The experimental results of this Section show that optically generated phonons can be used to study the transient broadening of the optical line shape of a single absorber. In principle, the dependence on the phonon frequency can be studied in such an experiment. In the same experiment the time-resolved dynamics of phonon diffusion and phonon decay in polymeric systems can be investigated via the dephasing mechanism of the optical probe.
6.4
Induced spectral diffusion
In this Section we will demonstrate that the resonant absorption of IR light in a polymeric system can also lead to irreversible line broadening phenomena. Even at a very low irradiation intensity (a typical value is 100 mW/cm2) the investigation of specific types of relaxation processes is possible. Such low irradiation intensities do not increase the temperature of the matrix by more than 0.01 K and hence yield no measurable dephasing effect via a change of the phonon distribution. Because of the irreversible nature of the optical line broadening, such phenomena are usually ascribed to spectral diffusion processes. The IR induced spectral diffusion is caused by addressing specific moieties within the matrix via the excitation of local vibrations. In the following weakly bound water molecules are studied. When a change in the spatial configuration takes place during the relaxation process of a water molecule the optical transition of a neighbouring dye molecule will be affected. Optical absorbers in glasses are therefore very sensitive probes for local rearrangements and are suited for a microscopic study of this topic. Due to the hydrophilic nature of the matrix the investigated guest host system, PMMA doped with H2Pc, contains a comparatively large number of water molecules (up to one volume percent). The experimental procedure is the following: A spectral hole is burned and its spectrum is repeatedly recorded while the sample is being exposed to IR radiation of a certain wavelength at a constant irradiation intensity. Figure 6.4 shows the typical increase of the hole
Figure 6.4: Time evolution of the hole broadening induced by different IR wavelengths. From top to bottom: 2.80 mm, 2.86 mm, 2.90 mm, 2.96 mm, and 3.04 mm.
83
6
Optically Induced Spectral Diffusion in Polymers Containing Water Molecules
Figure 6.5: Transmission spectra of PMMA without (curve A) and with (curve B) natural water content. The quotient C = B/A shows the H2O absorption lines. Dependence of the hole broadening on the IR wavelength after t0 = 35 min (curve D) due to induced spectral diffusion.
width and the strong dependence of this behaviour on the IR wavelength. To illustrate the pronounced spectral selectivity, one value of each hole broadening curve at t0 = 35 min is plotted in Fig. 6.5 (curve D) versus the corresponding IR wavelength. The data points do not simply reflect the absorption behaviour of the sample. Although the PMMA matrix has many absorption bands between 2 mm and 11 mm (curve B in Fig. 6.5), there are only two distinct wavelengths which give rise to induced spectral diffusion processes. The small concentration of water molecules in the matrix gives rise to non-saturated absorption bands near 2.8 mm and 6.1 mm. They correspond to the fundamental stretching and bending vibrations of H2O, respectively. The difference spectrum (curve C in Fig. 6.5) of water free and water saturated PMMA yields the exact position of the H2O absorption bands, which are in good agreement with the resonances found in our experiment. On an expanded scale in Fig. 6.5, even the asymmetric shape of the inhomogeneous H2O band is reflected by the experimental data. Replacing protonated with deuterated water yields a red shift of the IR resonances which also agrees very well with the corresponding absorption spectra of heavy water. In analogy to the tunneling model, which is based on the assumption of two potential minima, we assume two stable sites for each water molecule (Fig. 6.6). Since the experimental results indicate that a permanent change in the matrix occurs transitions between the two sites are only allowed via the first excited vibrational states. Using such a simple four-level model for the underlying kinetics, we are able to explain the temporal behaviour of the induced spectral diffusion in a quantitative fashion. 84
6.4
Induced spectral diffusion
Figure 6.6: Energy level scheme of a H2O molecule in a two-site model.
The two ground states are labelled 1 and 2, the first vibrationally excited states 3 and 4, respectively. The IR induced and the spontaneous transition rate for each site are denoted by the Einstein coefficients B and A, respectively. In our notation, B is proportional to the irradiated IR intensity. Transitions between the two sites are denoted by the conversion rate k. The transitions shown in Fig. 6.6 lead to a system of 4 coupled linear rate equations. Since we used in our experiments very low intensities of the IR light, we consider only the limit B P A where the population of the excited levels 3 and 4 is negligible at all times. The result is a time-dependent number of flips between the two ground states nf = n1?2 + n2?1 . Only those flips are taken into account which contribute to a change in the total configuration of all water molecules with respect to the time t = 0 of the hole burning process. According to Reinecke [7] the width of the spectral diffusion kernel Do is proportional to the number of flips nf . Though using the approximation that each flip yields the same contribution to Do, when taking into account the decrease of the IR intensity across the sample thickness as well as a random orientation of the H2O molecules, the result for Do can only be calculated numerically. Using a Taylor expansion, however, a very good analytical approximation of the width of the induced spectral diffusion is given by N0 !
t G 1 4pk
2Bpf t 1 b
b!
:
3
The difference between this formula and the numerical result is less than 5 %. pf is the flip probability of a single H2O molecule as defined by pf = k /(A + k), b is a dimensionless geometry parameter of about 2, N0 is the density of the H2O molecules and G is the coupling constant between dye and water molecules. Equation 3 describes very well the dependence of the broadening of a spectral hole on the number of absorbed IR photons (Fig. 6.4). It is possible to perform a test of the model. Equation 3 contains only two fitting parameters, the flip probability pf, and the coupling constant G. These two parameters can be obtained from a single experiment. An example is given in Fig. 6.7. One set of the experimental data (filled circles) is obtained at an IR intensity of 80 µW/cm2. The solid line is a fit according to Eq. 3 and yields a flip probability of 18 % and a coupling constant of G = 3.6 7 10–44 Jcm3. (Note: the slight difference with respect to the data given in reference [17] is due to the extension of the model by including the random orientation of the water molecules and the decrease of the IR intensity according to Beer’s law.) With these two values it is possible to calculate the 85
6
Optically Induced Spectral Diffusion in Polymers Containing Water Molecules
Time (s) Figure 6.7: Test of the model. Hole broadening versus IR irradiation time for three different IR intensities. The solid line is a fit, the dashed lines are calculated according to Equation 3.
time dependence of the induced spectral diffusion for any other irradiation intensity. The dotted lines in Fig. 6.7 are calculated with Eq. 3 for the obtained values and the intensities 230 µW/cm2 and 20 µW/cm2. The experimental results under these conditions, represented by the squares and triangles, are in very good agreement with the theoretical predictions. The high quantum yield of 18 % for the flip of a single water molecule becomes obvious by a comparison of the number of absorbed IR photons (typically 1014 s –1) with the total number of water molecules (about 1018) in the sample volume. Since a strong induced spectral diffusion is observed within several minutes, a local reorientation process with a high quantum yield must be involved. The coupling strength between water and dye molecules can be estimated by taking into account the static dipole moment of the H2O molecule. A reorientation of the H2O molecules affects the dye molecules by the concomitant change in the local electric field at the location of the chromophores. Assuming a mean distance of 15 Å and inserting data from Stark effect experiments [18], one obtains a value of approximately 2 7 10 –44 Jcm3 for the coupling constant which is very close to our fitted value. Together with the resonant phenomena discussed above, this yields a detailed microscopic understanding of this special kind of interaction. We can conclude that spectral diffusion induced by the absorption of IR photons in the frequency range 2–11 µm is a resonant process. Its microscopic origin is a spatial rearrangement of weakly bound water molecules after vibrational excitation. Assuming a configurational model with only two possible sites for each water molecule and applying the theoretical model of spectral diffusion by Reinecke [7], an analytical description of the resonant hole broadening behaviour can be obtained. A variation of the IR irradiation intensity shows that the model description yields excellent agreement with the experimental data.
86
References
References
1. 2. 3. 4. 5. 6.
7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18.
S. Jahn, K. P. Müller, D. Haarer: J. Opt. Soc. Am. B, 9, 925 (1992) M. Deye, P. Esquinazi: Zeitschr. für Phys. B, 39, 283 (1989) J. Friedrich, D. Haarer: Angew. Chem., Int. Ed. Engl,. 23, 113 (1984) C. A. Walsh, M. Berg, L. R. Narashiman, M. D. Fayer: Chem. Phys. Lett., 130, 6 (1986) J. M. Hayes G. J. Small: Chem. Phys., 27, 151 (1978) G. J. Small: Persistent nonphotochemical hole burning and the dephasing of impurity electronic transitions in organic glasses, in: V. M. Agranovich R. M. Hochstrasser (eds.): Spectroscopy and Excitation Dynamics of Condensed Molecular Systems, North-Holland, Amsterdam, p. 515 (1983) T. L. Reinecke: Sol. Stat. Com., 32, 1103 (1979) H. Maier, D. Haarer: J. Lumin., 64, 87 (1995) R. Greenfield, Y. S. Bai, M. D. Fayer: Chem. Phys. Lett., 170, 133 (1990) D. A. Parshin: Phys. Sol. State, 36, 991 (1994) U. Bogner: Phys. Rev. Lett., 37, 909 (1976) T. Attenberger, K. Beck, U. Bogner: in: S. Hunklinger, W. Ludwig, G. Weiss (eds.): Proc. of the 3rd Int. Conf. on Phonon Physics, p. 555 A. A. Gorokhovskii, G. S. Zavt, V. V. Palm: JETP Lett., 48, 369 (1988) W. Richter, Th. Sesselmann, D. Haarer: Chem. Phys. Lett., 159, 235 (1989) W. Richter, M. Lieberth, D. Haarer: JOSA B, 9, 715 (1992) G. Schulte, W. Grond, D. Haarer, R. Silbey: J. Chem. Phys., 88, 679 (1988) K. Barth W. Richter: J. of Lumin., 64, 63 (1995) R. B. Altmann, I. Renge, L. Kador, D. Haarer: J. Chem. Phys., 97, 5316 (1992)
87
7
Slave-Boson Approach to Strongly Correlated Electron Systems Holger Fehske, Martin Deeg, and Helmut Büttner
7.1
Introduction
The problem of understanding high-temperature superconductivity has been a challenge to theoreticians from a wide variety of fields. Many theoretical investigations have been carried out in order to identify the mechanism of this fascinating phenomenon as well as to establish the canonical model itself [1]. Although excellent progress is being made in deducing a consistent description of the high-temperature superconductivity systems from a first-principles theory, at present no microscopic theory can account for their unconventional normal-phase data in its entirety. The interplay of charge and spin dynamics in the normal state seems to hold the key to the understanding of the physical mechanism behind high-temperature superconductivity in the cuprates. Both macroscopic measurements of transport and magnetic properties as well as microscopic measurements probing the charge and spin excitation spectra are fundamental in establishing the anomalous normal-state properties of these materials [1]. The nature of spin excitations of the high-temperature superconductivity cuprates has been experimentally studied by means of nuclear magnetic/quadrupole resonance (NMR/ NQR) and inelastic neutron scattering (INS) techniques clarifying the persistence of strong antiferromagnetic (AFM) correlations in the normal and superconducting states [2]. Detailed investigations of the wave-vector dependence of the low-frequency spin fluctuation spectrum have revealed remarkable differences between the YBa2Cu3O6+x and La2–xSrxCuO4 families at low doping level x; the dynamic structure factor S (~ q, o) keeps its maximum at (p, p) in the YBCO system, while in LSCO, the peaks are displaced from the commensurate position to the four incommensurate wave-vectors p (1 + q0, 1), p (1,1 + q0), where q0 F 2x. On the other hand, the analysis of the NMR data shows that the relaxation rates on the planar Cu sites are similar in all materials. Two striking features are associated with 63T 1–1 : a) as a result of strong local spin fluctuations on 63Cu sites it is enhanced by one order of magnitude over the oxygen rate 17T 1–1 ; and b) in sharp contrast to the Korringa-like behaviour at the planar 17O sites, its temperature dependence does not follow the Korringa law [2]. 88
Macromolecular Systems: Microscopic Interactions and Macroscopic Properties Deutsche Forschungsgemeinschaft (DFG) Copyright © 2000 WILEY-VCH Verlag GmbH, Weinheim. ISBN: 978-3-527-27726-1
7.1
Introduction
The physical origin of the contrasting q~-dependence of the spin fluctuation spectrum is still under discussion. Millis and Monien [3] have argued that the spin dynamics and, in particular, the temperature dependence of the spin susceptibility ws (T) in LSCO are caused by a spin density wave instability, whereas in the YBCO family they are due to in-plane AFM fluctuations and a novel non-Fermi liquid spin singlet pairing of electrons in adjacent planes. On the other hand, the magnetic properties are intimately related to the energy band dispersion of the non-interacting system within a Fermi liquid based framework, i. e., in this way the observed spin dynamics can be attributed to different Fermi surface (FS) geometry of LSCO-type and YBCO-type, respectively. Along this line, details of the spin fluctuation spectrum are studied using a nearly antiferromagnetic Fermi liquid approach by Monthoux and Pines [4]. From a more microscopic point of view, the important effects of FS shape on the magnetic properties were confirmed by Si et al. [5] within a large Coulomb-U auxiliary boson scheme and by Fukuyama and co-workers [6] on the basis of a resonating valence bond (RVB) slave-boson mean-field approach to the extended t-J model. Furthermore, Ito et al. [7] have recently reported that the charge transport in the CuO2 plane is determined by dominant spin scattering, i. e., the spin dynamics are manifest in the extraordinary transport properties of the high-temperature superconductivity cuprates as well. Encouraged by these findings it is the aim of this report to study magnetic and transport phenomena of high-temperature superconductors probably in terms of the most simple effective one-band model describing both correlation and band structure effects, the socalled t-t'-J model: Ht
t0 J
t
X hi;ji;
c~yi c~j
t0
X hhi;j ii;
c~yi c~j J
X hi j i
S~i S~j
n~ i n~ j 4
:
1
Ht–t'–J acts in a projected Hilbert space without double occupancy, where c~
y i = P y 1 ~ n~i is the electron annihilation (creation) operator, Si 2 0 c~i ~ 0 c~i 0 ; and n~ i c~yi c~i . J measures the AFM exchange interaction, t and t' denotes hopping processes between nearest-neighbour (NN; Ai,jS) and next nearest-neighbour (NNN; AAi,jSS) sites on a square lattice. Compared to the original t-J model the t'-term incorporates several important effects near half-filling. Starting from a rather complex three-band Hubbard or Emery model [8] for the CuO2 planes, quantum cluster calculations [9] have revealed that the relative large direct transfer between NN oxygen sites (tpp < tpd /2) leads to a sizeable NNN hopping t' in the context of an effective one-band description. More recently the t'-term has been introduced to reproduce the FS geometry observed in ARPES experiments [6, 10–12]. Fitting the quasi-particle dispersion relation c
y i
1P
"k~
2t
cos kx cos ky
4t0 cos kx cos ky ;
2
involved in Eq. 1 to experimental and band theory results yields t in the order of 0.3 eV and, e. g., for the case of YBCO, t' & –0.4 t [4, 5, 13]. Moreover, Tohyama and Maekawa [12] have emphasized that a t-t'-J model with t' > 0 can be used to describe the electron-doped systems, e. g. Nd2–xCexCuO4 (NCCO). In this case one has to shift the momentum k~ ? k~ + (p, p) [12], i. e., within a band-filling scenario one obtains a hole pocket-like FS centred at (p, p)-point which shrinks with increasing doping [14]. Finally, as pointed out by Lee [15], 89
7
Slave-Boson Approach to Strongly Correlated Electron Systems
in a locally AFM environment doped holes can propagate coherently only on the same sublattice without disturbing spins. Therefore, the t'-term coupling the same sublattice becomes crucial for the low-lying magnetic excitations. This clearly is a correlation effect related to the NNN hopping processes.
7.2
Slave-boson theory for the t-t'-J model
Apart from numerical techniques, the slave-particle methods have been employed extensively in studying the effects of electron-electron correlation in the (extended) t-J model [6, 16–21]. The two commonly used approaches, the NZA slave-boson [16, 17] and slave-fermion [18] schemes, however, yield quite different results concerning the (mean-field) ground-state phase diagram and spin/charge excitations for this model [22]. As yet, the relationship between both types of slave-field theories is not well understood. Within the NZA formulation, for example, the Hamiltonian can be solved by a mean-field approximation with the (uniform) RVB order parameter. A serious difficulty of this approach is the absence of AFM correlations [18, 22], e. g., in the half-filled case, the lowest energy state, the energy of which is considerable higher than numerical estimates indicate, does not satisfy the Marshall sign rule and fails to show the expected long-range Néel order [23]. On the other hand, the mean-field slave-fermion schemes [18] are known to give reasonable results for the spin susceptibility as well as for the spin correlation length [21, 22], but also suffer from neglecting important correlation effects, especially the fermion charge degrees of freedom are not described sufficiently well. In contrast, the fourfield slave-boson (SB) technique, introduced by Kotliar and Ruckenstein (KR) [24] in the context of the Hubbard model, has the advantage of treating spin and charge degrees of freedom on an equal footing. Starting from the scalar KR SB representation of the Hubbard model, one may generate an intersite exchange interaction via a loop expansion in the coherent state functional integral [19]. However, the effective t-J Lagrangian, derived in this way, contains only an Ising interaction term, i. e., important spin-flip exchange processes are neglected. As we shall see below, to bosonize the complete exchange interaction term one has to use the spin-rotation-invariant (SRI) extension of the KR SB theory from the beginning [25, 26].
7.2.1 SU(2)-invariant slave-particle representation For the sake of definiteness, we return to the extended t-J Hamiltonian (Eq. 1), that may be cast into the form Ht
t0 J
X i;j
90
~ yi ~j tij
J X ~ y ~ ~ y ~ i i j j : 4 hi j i
3
7.2
Slave-boson theory for the t-t'J model
In order to bring out the SU(2) symmetry of the system, we have used in Eq. 3 a spinor ~ yi
~ yi ; ~ i ~ i are built up representation, where the one-row [one-column] matrices y y ~ ~ by the projected fermion creation [annihilation] operators i c~i i c~i : denotes the contravariant [covariant] four-component vector (m = 0, x, y, z) of Pauli’s matrices. To preserve SRI, we apply to Ht-J the manifest [SU(2) 6 U(1)] invariant SB scheme [26, 27] based on the SRI SB approach developed for the Hubbard model by Li et al. [28]. Accordingly, we define scalar boson fields e({) and bosonic matrix operators p({) (representing i i empty and singly occupied sites, respectively) and pseudofermion spinor fields C({) in the i following way: j0i i eyi jvaci ; j i i
X
yi pyi jvaci :
4
The unphysical states in the extended Fock space of pseudofermionic and bosonic states are eliminated by imposing two sets of local constraints: Ci
1 eyi ei 2Trpyi pi
1 0;
5
expressing the completeness of the bosonic projectors, and y y C
2 i i i 2pi pi
o 0 ;
6
relating the pseudofermion number to the number of p-type slave-bosons (hereafter underbars denote a 262 matrix in the spin variables). Obviously, double occupancy has been projected out. In the transformation of the fermionic spinor fields analogous to [26, 28], ~ ! zi i ; i
7
the non-linear bosonic hopping operators zi o
2pyi pi
1=2 y ei 1
eyi ei 2Trpyi pi 1=2 pi
1
eyi ei o
2p~ yi p~ i
1=2
8
({) yield a correlation-induced band renormalization where p~ ({) irr' = rr'pi, –r',r . Exploiting the SU(2),O(3) homomorphism, the matrix operators pi may be decomposed into scalar (sing~i = (pix , piy, piz) components as let) p({) o and vector (triplet) p
p
y i
1X p
y ; 2 i
9
where the pim obey the usual Bose commutation rules pi; pyj0 ij 0 . Consequently, the pseudofermions i
i ; i T satisfy anticommutation relations of the form f i ; yj0 g ij 0 . 91
7
Slave-Boson Approach to Strongly Correlated Electron Systems
This way the interaction term is converted due to ~ i ! 2Tr pyi p ; ~ yi i
10
where, more explicitly, the locally defined particle number and spin operators are just n~ i ! n~ i
pi 2Trpyi pi
P
pyi pi ;
1 S~i ! S~i
pi Trpyi ~pi
pyio p~i p~yi pio 2
ip~yi p~i :
11
Actually, the components of the bosonized SB spin operator act as generators of rota
2 tions in spin space, i. e., S~i
pi satisfies the spin algebra. Since C(1) commute with i and C i the SB t-J Hamiltonian, the constraints in Eq. 5 and Eq.P 6 can be ensured by introducing the
2 1 time-independent Lagrange multipliers i
1 and
2 i i . As a consequence, the Hamiltonian of the t-J model (Eq. 3) in terms of the slave-boson and pseudofermion operators has to be replaced by HSB t t0
J
P i;j
tij yi zyi zj j
P i
i
1 Ci
1
J
P
Tr pyi pi
hi j i
2 Tr
2 i Ci :
Tr pyj pj
12
In the physical subspace, HSB t–J possesses the same matrix elements for the basis states (Eq. 4) as the original t-J Hamiltonian (Eq. 3) for the purely fermionic states. To verify this directly, special attention has to be paid to the bosonization of AFM exchange interaction term
~ yi ~i
y P ~ j 2
c~yi c~yj c~ c~ ~ j j i
c~yi c~yj c~j
c~i
;
13
which includes besides the Ising exchange contributions #i "j $ #i "j the spin-flip processes #i "j $ "i #j . Let us emphasize that the matrix elements of the spin-flip terms are not reproduced in the scalar KR SB approach [19]. By contrast, within the SRI SB approach it is a straightforward exercise to show that these contributions can be expressed in terms of the p({) irr' : X 0
pyi pyj0
pj0 pi
i j 1 i 4
j :
14
Thus our SRI SB scheme (Eqs. 4–12) provides a consistent bosonization of the extended t-J model. 1 Note that additional constraints do not exist. Especially, if the constraint p~i p~i 0 is added [25] the spin algebra is not satisfied.
92
7.2
Slave-boson theory for the t-t'J model
7.2.2 Functional integral formulation To proceed further, it is convenient to represent the grand canonical partition function for the redefined SB Hamiltonian (Eq. 12) in terms of a coherent-state functional integral [29] over Grassmann fermionic and complex bosonic fields as R Z dL
1
2 ; De ; e Dp p d d e 0 Z D ; ; L
P
1 T ei
@
1 i ei 2Tr pi
@ i o i
P hi;ji P i
Trpi ~pi Tr pj ~pj
i
@
Tr pi pi Tr pj pj
T
2 pTi i
1 i
P i z zj j : o i
2 i ti j i i;j
15
16
Apart from the above symmetry considerations the SB functional-integral formalism reveals additional global R and local gauge invariances [25, 30–32]. The action S 0 dL
is invariant under the following site and time-dependent phase transformations (yi (t)wi (t)), i. e., under the local symmetry group SU(2) 6 U(1), i ! e
ii ii
e i ;
e i ! ei e
ii
pi ! pi e
i
; i
17
;
provided that the (five) Lagrange parameters act as time-dependent gauge fields, l(1) i (t) and l
2 i
t, absorbing the time derivatives of the phase factors: _ !
1
1 i i i i ; i
2 i
2 i ! e i e
i
i
i_ i i_i o :
18
Next, in the continuum limit, the radial gauge is introduced by representing the Bose fields by modulus and phase, ei jei jei'
ei ; pi
1 X i
p pi e i ; 2
19
93
7
Slave-Boson Approach to Strongly Correlated Electron Systems
(for a time-discretized version of this gauge fixing, see [31]). Exploiting the gauge freedom of the action, we can now fix the five real-valued coefficients yi (t), wim (t) to remove five phases (ji (t), fim (t)) of the Bose fields ei, pim in the radial gauge. As a consequence, all the Bose fields {ei, pim} become real, in contrast to the Hubbard model, where one SB field remains complex [25, 32]. At this point P one should notice that the particle number and spin operators are changed into n~ i
pi p2i ; S~i
pi pio p~i (the previous notations ei, pio and p~i now denote the radial parts of the corresponding Bose fields). Then, using the familiar identity for Gaussian integrals over Grassmann fields [29], R
G 1 0
; e D
G 1
eTr ln
;
20
the fermionic degrees of freedom can be integrated out and we obtain the following exact representation of the grand canonical partition function Z
R
Sef f
D e
21
in terms of the real-valued bosonic fields fia,
2
2
2 ; i
1 ; pix ; ix ; piy ; iy ; piz ;
2 i
i
ei ; pio ; io iz :
22
In Eq. 21 the effective bosonic action Seff takes the form Sef f
R
d
( P i
0
J
P
2
1 i ei
hi j i
pio p~i p~j pjo
P
1 i
2
2 io pi
2pio p~i ~
2 i
1 2
p p~2i
p2jo p~2j 4 io
i
1
)
h i 1 0 Trij;0 ;0 ln Gij; 0
; ;
23
where the (inverse) SB Green propagator is given by 1 0 Gij; 0
;
h
@
2 io 0
tij
zyi zj 0 ;0
1
ij :
i ~0 ij
~
2 i
0
24
It may be remarked that since the bosons are taken to be real, their kinetic terms, being proportional to the time derivatives in Eq. 16, drop out due to the periodic boundary conditions imposed on Bose fields (fia (b) = fia (0)). Strictly speaking it follows from this property that all the Bose fields do no longer have dynamics of their own [25].
94
7.2
Slave-boson theory for the t-t'J model
7.2.3 Saddle-point approximation The evaluation of Eq. 23 proceeds via the saddle-point expansion 2, where at the first level i of the bosonized action Seff with respect of approximation we look for an extremum S
to the Bose and Lagrange multiplier fields fia : @Sef f ! 0 ) S Sef f i i : @i
25
i is determined to give the lowest free energy The physically relevant saddle-point F (per site) ft
t0 J
=N n ;
26
where at given mean electron density n = 1 – d, the chemical potential m is fixed by the requirement n
1 @
N @
27
S= denotes the grand canonical potential). Obviously, an unrestricted minimization of (O the free energy functional is impossible for an infinite system. To keep the problem tractable, we use the ansatz ~ i m~ m ui ;
u~i
cos Q~ R~i ; sin Q~ R~i ; 0
28
~ i 2S~i 2pio p~i . Following earlier analyses of spiral states for the local magnetization m for the Hubbard model [34] the unit vector u~i is chosen as a local spin quantization axis pointing in opposite directions on different sublattices. Thereby, the order parameter wavevector Q~ is introduced as a new variational parameter to describe several magnetic ordered states: PM, FM (Q~ = 0), AFM (Q~ = (p,p)), and incommensurate (1,1)-spiral (Q~ = (Q, Q)), (1,p)-spiral (Q~ = (Q,p)) and (0,1)-spiral (Q~ = (0,Q)) states. Note that since fluctuations of the charge density are not incorporated the scalar Bose fields are homogeneous: ei = e, pio = (1) (2) (2) po, l(1) i = l , and lio = lo . The vector fields exhibit the same spatial variation as the mag
2 ~ ~ o)-representation netization: p~i p~ ui and li l
2 u~i . Then transforming Eq. 23 in the (k; the trace in Seff can be easily performed to give the free energy functional
2 Mean-field approximations to the functional integral are achieved by replacing the bosonic fields by their time averaged values. For the Hubbard model, a comparison of the paramagnetic and antiferromagnetic SB solutions with quantum Monte Carlo results shows that such a mean-field like approach yields an excellent quantitative agreement for local observables [33] and therefore can give a qualitative correct picture with relatively little effort.
95
7 ft
t0 J
Slave-Boson Approach to Strongly Correlated Electron Systems
2 2
1
e2 p2o p2 1
2 2
2 po p n o
po p 1 2
po p2 2 J p2o p2
cos Qx cos Qy 2
1 X ln1 N ~
nk ~ ;
29
1
30
k
where nk ~ exp f
Ek ~
g 1
holds. The renormalized single-particle energies Ek ~
are obtained by diagonalizing the kinetic part of Eq. 23 [26]. Requiring that ft-J be stationary with respect to the variation of the magnetic order vector, the wave-vector Q~ can be obtained from the extremal condition sin Qx;y
@Ek 1 1 X ~ nk : ~ 2 2 Jpo p N ~ @Qx;y
31
k
If one substitutes Eq. 31 together with f a (obtained from the solution of the coupled self-consistency equations (Eq. 25)) into Eq. 29, the free energy of the t-t'-J model is obtained as ft
t0 J
J 2 m
cos Qx cos Qy 4 1 X ln 1 e
Ek~ N ~
2n2
2 m
2 o n
;
32
k
where the quasi-particle energy takes on the form
2 Ek ~
1
"k~ "k~ Q~ =y o h 2
"k~ "k~ Q~ 2 =y m
"k~ "k~
=y Q~
2 2
i1=2
33
with m = 2 po p and y = (1+d)2 – m2.
PM = (e, po, l(2) In particular, at the spatially uniform paramagnetic saddle-point, F o , (1) l ; 0, 0; 0, 0; 0, 0) the remaining bosonic fields e2 ;
96
p2o 1
;
1
2 3 2 "~
0 ; 1 2
2 o
2 "~
0
1 2
1
J ;
34
7.2
Slave-boson theory for the t-t'J model
are explicitly given in terms of J, d and a single energy parameter "~ (0) defined by "~
~ q
2 X " N ~ k~
q~
Ek~
35
k
(at T = 0). Here, the quasi-particle energy Ek~ is Ek~ 2"k~=
1
2 0 ;
36
and m can be determined from d = 1 – free energy becomes simply 2 f
PM t t0 J z "~
0
1 J
1 2
2 N
P
2
1
k~
Ek~. Finally, in this approximation, the
:
37
7.2.4 Magnetic phase diagram of the t-t'-J model In the numerical evaluation of the self-consistency loop we proceed as follows: at given model parameters J and d, we solve the remaining saddle-point equations for m, l(1), l(2) o and l(2) together with the integral equation for m using an iteration technique. Then, in an outer loop, the order parameter wave-vector Q~ is obtained from the extremal Eq. 31 by means of a secant method. Convergence is achieved if all quantities are determined with relative error less than 10 –6. Note that our numerical procedure allows for the investigation of different metastable symmetry-broken states corresponding to local minima of the variational free energy functional (Eq. 32). At first, let us consider the case t' = 0, i. e., the pure t-J model. The resulting groundstate phase diagram in the J-d plane is shown in Fig. 7.1. For the case d = 0 (Heisenberg model), we obtain an AFM ground state. At J = 0, the FM is lowest in energy up to a hole concentration of 0.327, where a first-order transition to the (1, p)-spiral takes place; above d = 0.39, we find a degenerate ground state with wave-vector (0, p). At d = 0.63 the PM becomes the lowest in energy state (second-order transition). This coincides with the U ? ? SB results of the Hubbard model (J = 4t2/U) [35]. The PM-FM instability occurs at dPM-FM = 0.33 [32]. In contrast, the slave-fermion phase diagram [20] exhibits a much larger FM region. This can be taken as an indication that correlation effects are treated less accurate within the slave-fermion mean-field scheme [20, 36]. For finite exchange interaction J the (1,1)-spiral is the ground state at small doping. With increasing d a transition to the FM takes place, which becomes unstable against the (1, p)-spiral at larger doping concentrations. For J/t > 0.08, we find a transition from (1,1)-spirals to (1, p)-spirals at about d & 0.2. In Figure 7.1, the dotted line separates the (1, p)-spiral state from the region, where the (1, p) and (0, p) states are degenerate. If we admit only homogeneous phases, the phase boundaries (1,1)-spiral ⇔ (1, p)-spiral at d & 0.2 and (1, p)/(0, p)-phase ⇔ PM at d & 0.63 remain nearly unchanged at larger values of J. However, analyzing the thermodynamic stability of 97
7
Slave-Boson Approach to Strongly Correlated Electron Systems
Figure 7.1: SB ground-state phase diagram of the t-J model.
the saddle-point solutions (i. e. the curvature of ft J
d), one observes a tendency towards phase separation into hole-rich and AFM regions above the ‘diagonal’ solid curve in the left upper part of the J-d phase diagram (see below). Figure 7.2 displays the variation of the extremal spiral wave-vector Q~ as function of doping. At d = 0, Q~ = (p, p) indicates the AFM order. At low doping the (1,1)-spiral order vector decreases approximately linear. With decreasing J the AFM exchange is weakened, consequently the deviation of the order vector from (p, p) increases. The discontinuities reflect the first-order transition from (1,1)-spirals to (1, p)-spirals. For J/t = 0.05 the transition to the FM state takes place, with Qx jumping down to zero. The (1, p)-spiral wave-vector shows a monotonous decrease of Qx until at d = 0.63 the transition to the PM (Qx = 0) occurs. Comparing the magnitude of the theoretical order vector of the spiral solutions to results from inelastic neutron scattering experiments on La2–xSrxCuO4 [37], we find good agreement for an exchange interaction strength of J/t = 0.4 (which seems to be a reasonable value with respect to the strong electron correlations observed in the high-temperature superconductors).
~ as a function of doping d (compared with exFigure 7.2: The x-component of the spiral wave-vector Q periments [_] on LSCO [37]).
98
7.2
Slave-boson theory for the t-t'J model
Next, we investigate the ground-state properties of the t-t'-J model, where we fix J/t = 0.4. Comparing the free energies of several (homogeneous) symmetry-broken states, we obtain the SB phase diagram shown in the t'/t-d plane in Fig. 7.3. Obviously, we can distinguish two regions. In the parameter region |t'/t| ^ 0.2, Figure 7.3 resembles the groundstate phase diagram of the pure t-J model (Fig. 7.1), i. e., we found large regions with incommensurate spiral order. However, compared to the pure t-J model, the t'-term stabilizes Néel order in a finite d region near half-filling. The increasing stability of AFM configurations can be intuitively understood because the t'-term moves electrons without disturbing the Néel-like background [12]. For larger ratios |t'/t| we have a completely different situation. In this parameter regime only commensurate states (AFM, FM, PM) occur, where for t' < t'c = –1.4 t we obtain the AFM state for all d. Note the rather large differences to the value of t'c obtained within a semiclassical (1/N)-expansion [38]. By varying the exchange coupling J, the phase boundaries in the t'/t-d plane are not much affected, e. g. for J/t = 1 and t'/t = –0.4, the transitions AFM ⇔ (1,1)-spiral and (1,1)-spiral ⇔ FM take place at d = 0.17 and d = 0.6, respectively. We would like to point out that the main qualitative features of our SB phase diagram do confirm recent studies of magnetic long-range order in the t-t'-J model [38, 39].
Figure 7.3: Restricted SB ground-state phase diagram of the 2D t-t'-J model at J/t = 0.4.
In Fig. 7.4 we plot the order parameter wave-vector as a function of doping at t'/t = +0.16 and t'/t = –0.4. The behaviour of Qx reflects a series of transitions AFM ⇔ (1,1)spiral ⇔ (1, p)-spiral ⇔ PM. The corresponding (sublattice) magnetization abruptly changes at the (1,1)-spiral ⇔ (1, p)-spiral first-order transition. From Fig. 7.4 the asymmetry between hole (t' < 0) and electron doping (t' > 0) becomes evident. In contrast to recent HartreeFock results for the Hubbard model [40] we found the AFM phase near half-filling for both electron-doped and hole-doped cases (provided t' ( 0). In the absence of t ' hopping, for arbitrarily small doping the AFM is found to be unstable against the (1,1)-spiral phase (cf. Fig. 7.3). Obviously, the AFM correlations are strongly enhanced by a positive t'-term, which is also in qualitative agreement with exact diagonalization studies of the t-t'-J model [12] and confirms the experimental findings for the electron-doped system NCCO [41, 42]. Note that the stability region of the AFM phase agrees surprisingly well with the combined 99
7
Slave-Boson Approach to Strongly Correlated Electron Systems
~ away from half-filling for the negative vaFigure 7.4: The x-component of the SB spiral wave-vector Q lues t'/t = –0.16 (solid) and t'/t = –0.4 (long-dashed), i. e., hole doping (d > 0), and for the positive one t'/t = 0.16 (dashed), i. e., electron doping.
phase diagram for La2–xSrxCuO4 and Nd2–xSrxCuO4 obtained from neutron scattering [43] and muon spin relaxation measurements [44], respectively. For the YBCO parameter t'/t = –0.4, the AFM disappears around d = 0.1 whereas in the phase diagram of YBCO, determined by neutron diffraction [45], this transition takes place at about x = 0.4 oxygen content. However, there exits strong evidence that at least up to x = 0.2 no holes are transferred from CuO chains to CO2 planes. As we have already noted, the phase diagrams in Fig. 7.1 and Fig. 7.3 result from the relative stability of various homogeneous states. On the other hand, there are arguments for the existence of inhomogeneous, e. g., phase-separated states in the t-J and related models [46]. Using very different methods, it was realized by several groups [47–51], that at large J/t the ground state of the t-J model separates into hole-poor (AFM) and hole-rich regions. Unfortunately, in the physically interesting regime of small exchange coupling (J/t ~ 0.2– 0.4) and low doping level this point is still controversial. To gain more insight into the phenomenon of phase separation in t-J-type models of strongly correlated electrons it seems to be important to investigate the effect of an additional NNN hopping term t' as well. Therefore we study the free energy as a function of hole density d, where a (concave) convex curvature indicates local thermodynamic (in)stability implying a (negative) positive inverse iso@2 f –1 thermal compressibility k–1 = n2 @n < 0, the domain of the two-phase regime is deter2 : If k mined performing a Maxwell construction for the anomalous increase of the chemical potential m by doping. The results of our analysis of thermodynamic stability are depicted in Figs. 7.5 a and 7.5 b for the t-J and t-t'-J model, respectively. The boundary of phase separation for the t-J model is given by the solid curve in the J-d plane shown in Fig. 7.5 a. As can be seen from Fig. 7.1, the different phase separated domains are built up by the (AFM) states at half-filling (d = 0) and the corresponding hole-rich state on the right boundary of the respective region. At J = 0, where we recover the U ? ? result of the Hubbard model [32], the free energy is a convex function Vd, i. e., our SRI SB theory does not support recent arguments [47] for phase separation in this limit. In the opposite limit of large J, complete charge se100
7.2
Slave-boson theory for the t-t'J model
Figure 7.5: Phase diagram of the t-(t')-J model including phase separated states. The phase separation boundary (solid curve) for the t-J model is shown in the J-d plane (a). We include the transition lines of Refs. [49] (dashed), [50] (dotted), and [51] (chain dashed). The triangles are the Lanczos results of Ref. [47]. The phase diagram of the t-t'-J is calculated in the t'/t-d plane at J/t = 0.4 (b). Here the twophase region consists of AFM and (1,1)-spiral states. For further explanation see text.
paration takes place for J/t > JPS /t = 4.0, which seems to be an essentially classical result. From exact diagonalization (ED) we obtain JPS /t = 4.1 + 0.1 [52] compared with 3.8 derived by means of a high-temperature expansion [51]. We note that the homogeneous magnetic phases are always unstable close to half-filling (provided J/t > 0). This is in qualitative agreement with results obtained from ED studies [47] as well as from semiclassical [49] or renormalization-group calculations [50]. Also plotted in Fig. 7.5 a are the results of the hightemperature expansion method [51], where phase separation may occur only above a critical exchange J/t = 1.2 as d ? 0, contrary to all the other approaches. The line separating the two-phase region from the stable states was determined by Marder et al. [49] within a semiclassical theory to vary as J/t = 4 d2 whereas our theory yields an approximately linear dependence at small d. We believe that, due to an improved treatment of spin correlations in our approach, the region of incomplete phase separation is reduced. The instability towards phase separation at small J can be taken as an indication that charge correlations may play an important role as well. The dotted lines of zero inverse compressibility in Fig. 7.5 b show that also for |t'/t| > 0 there is a finite range of d over which the (1,1)-spiral is locally unstable. Similar results were recently obtained by Psaltakis and Papanicolaou [38]. But it is important to stress that in our theory the AFM state is locally stable for both signs of t'. In addition, based on the Maxwell construction, we can show that near half-filling the AFM state remains also globally stable against phase separation for the t-t'-J model (cf. Fig. 7.5 b, where the two-phase region is bounded by the solid lines). At larger values of |t'/t| 6 0.5, the phase-separated region is due to the first-order nature of the transition AFM ⇔ (1,1)-spiral (dashed curve) [38]. Finally to demonstrate the quality of our SRI SB approach, for the t-J model the expectation value of the kinetic energy is compared with the results from ED for a finite 16site [48] (36-site [52]) lattice in Fig. 7.6. We find an excellent agreement between SB results and ED data. Obviously, this result does not depend on the interaction strength J, i. e. the SB 101
7
Slave-Boson Approach to Strongly Correlated Electron Systems
Figure 7.6: Expectation value of the kinetic energy as a function of doping at several interaction strengths J in comparison to ED results for the 16 (36) site lattice [48, 52].
theory well describes important correlation effects. Note that AHtSt–J /t is directly related to the effective transfer amplitude of the renormalized quasi-particle band, which is taken as input for the calculation of transport coefficients in the following section.
7.3
Comparison with experiments
7.3.1 Normal-state transport properties As one of the main normal-state puzzles of the CuO2 based high-temperature superconductors, the anomalous transport properties, in particular the temperature and doping dependence of the Hall resistivity RH (T, d) [53–56], has been under extensive experimental and theoretical study. Quasi-particle transport measurements suggest a small density of charge carriers and hence a small pocket-like Fermi surface (FS) [57]. On the other hand, direct angle-resolved photoemission (ARPES) probes of the FS [14, 58] yield a large FS which satisfies Luttinger’s theorem and might be well described by (LDA) band structure calculations [13, 59]. In principle, this contrasting behaviour is found for hole-doped (La2–xSrxCuO4, YBa2Cu3O6+x) and electron-doped (Nd2–xCexCuO4) copper oxides as well. Adopting the hypothesis of Trugman [60], most of the normal-state properties of the cuprates may be explained by the dressing of quasi-particles due to magnetic interactions and the subsequent modification of their dispersion relation. Then, once the quasi-particle band Ek ~ has been obtained, the Hall resistivity RH = sxyz /sxxsyy can be calculated in the relaxation time approximation, using standard formulas for the transport coefficients: 102
7.3 Comparison with experiments
@nk e2 X ~ uk ; ~ u k ~ 2 @E k V ~ ~ k k
(38)
@u k ~ @nk e X ~ uk : ~ " uk ~ 4 @k @Ek k cV ~ ~ 3 2
k
Here nk ~ is given by Eq. 30, V denotes the volume of the unit cell, elkg is the completely antisymmetric tensor, and uk ~ =@k . Note that RH does not depend on the relaxa~ @E k tion time t. To make the discussion more quantitative, let us now consider the doping dependence of RH (d,T ) in terms of the t-t'-J model using the saddle-point and relaxation time approximations, where FS and correlation effects are involved via the renormalized SB band Ek ~ (Eq. 33). As we have pointed out above, in our approach the SB quasi-particle band dispersion Ek ~ has to be determined in a self-consistent way at each doping level d. This should be in contrast to the NZA SB mean-field approach to the t-t'-J model of Chi and Nagi [61] where, in the J ? 0 limit, the calculation of transport properties is based on the simple replacement "k~ ! "~k~ = –2 td [(cos kx + cos ky) + 2 (t'/t) cos kx cos ky] of the non-interacting band dispersion (Eq. 2). Figure 7.7 shows the theoretical Hall resistivity as a function of carrier density in comparison to experiments on LSCO [53], YBCO [54] and NCCO [55, 56]. In the LSCO and NCCO systems, the concentration of chemically doped charge carriers in the CuO2 planes (d) definitely agrees with the composition (x) of the substitutes Sr and Ce. This simple relation, however, no longer holds for YBCO, i. e., the number of holes transferred into the planes does not increase linearly with the oxygen content. Indeed, the magnetic properties indicate d & 0 up to x = 0.2 [45]. In order to compare our theoretical model with the RH (x) data found on oxygen-doped YBCO, we use the relation d = (x – 0.2)/2 [62].
Figure 7.7: Doping dependence of the Hall resistivity for hole-doped (left panel) and electron-doped (right panel) systems. The slave-boson results for J/t = 0.4 and different ratios t'/t = 0 (solid), –0.16 (dashed), –0.4 (chain dotted) and t'/t = 0.16 (dotted) are compared with experiments on LSCO (_) [53] (at 80 K), YBCO (O) [54] (at 100 K) and NCCO (Z) [55, 56] (at 80 K), respectively. The inset shows the temperature dependence of RH for t'/t = 0 at d = 0.1 (short dashed) and d = 0.15 (dotted).
103
7
Slave-Boson Approach to Strongly Correlated Electron Systems
Figure 7.7 clearly demonstrates the importance of the NNN transfer term t' for a consistent theoretical description of the experimental Hall data. For J/t = 0.4, an excellent agreement with experiments on LSCO and NCCO, including the sign change of RH (d) at a very similar value, can be achieved using the parameter values t'/t = 0 and t'/t = 0.16, respectively. It should be noted that in the case of LSCO we obtain t'/t = 0 from RH (d) while LDA calculations yield a ratio t'/t = –0.16 [13, 59]. For YBa2Cu3O6+x, where the experiments [54] give RH > 0 up to x = 1, a negative t'-term suffices to give the correct tendency to RH (d). Using t'/t = –0.4, our theory yields a sign change of RH at d & 0.7. The strong increase (decrease) of the positive (negative) Hall coefficient as d ? 0 can be attributed to the formation of small hole (electron) pockets in the FS, which is a correlation effect. A recent analysis of resistivity saturation in LSCO [57], based on Boltzmann transport, has been taken as an indication of a small FS as well, however, the existence of a pocket-like FS is still a subtle and unresolved issue. We found that the temperature dependence of RH (d,T ) is at least in qualitative agreement with experiments on LSCO (see inset Fig. 7.7 (left panel)). Note that the quasi-particle dispersion Ek ~ exhibits extremely flat minima implying the presence of a new small energy scale D. Therefore, when the temperature becomes comparable to D the hole pockets are washed out and a sign change of RH occurs (cf. Fig. 7.7 at fixed d (inset)). 3 The FS of the interacting system are shown in Fig. 7.8 for typical ratios t'/t at J/t = 0.4 and d = +0.1, where the diagonal (1,1)-spiral phase is lowest in energy. As observed for t-J and Hubbard models as well [64], we obtain small hole (or electron) pockets with a volume ! |d|. The calculated FS are very anisotropic. As |d| increases, the pockets grow, until the FS topology changes completely at a critical doping value dc (RH (dc) = 0 (cf. Fig 7.7), reflecting the transition from hole to electron carriers for t'/t < 0 and vice versa for t'/t > 0.
Figure 7.8: Quasi-particle Fermi surface in the (1,1)-spiral phase at J/t = 0.4 for d = 0.1 (hole-doped system) and d = –0.1 (electron-doped system).
3 We recently learned of a related exact diagonalization study of Dagotto et al. [63], where, similar in conclusion, the doping and temperature dependence of RH was calculated using a strongly renormalized flat quasi-particle dispersion.
104
7.3 Comparison with experiments We want to point out that the renormalization of the quasi-particle band Ek ~ strongly depends on both interaction strength J and doping level d [62] which, in fact, calls into question the frequently used rigid band approximation. Due to the strong coupling of spin and charge dynamics the characteristic energy scale for the coherent motion of the charge carriers is J and not t (provided t > J).
7.3.2 Magnetic correlations and spin dynamics In this Section we try to understand the INS and NMR experiments on the basis of the SRI SB mean-field theory. Using a generalized RPA expression for the spin susceptibility and assuming that the AFM correlations are spatially filtered by various q~-dependent hyperfine form factors, we focus, in particular, on the spin dynamical properties in the paraphase of the t-t'-J model. Our starting point is an RPA-like form for the exchange-enhanced spin susceptibility [5, 6, 65] o
~ q; !
s
~ q; ! 1
J
cos qx cos qy o
~ q; ! 2
:
39
The irreducible part 4 2 X ~ k~ q~; i!nm G
k; i!n G
N ~
o
~ q; i!m
40
k;n
~ i!n i!n E ~ ~ 1 describing noncontains the (dressed) SB Green propagators G
k; k interacting electrons with the renormalized band structure Ek~
d (Eq. 26). Once the dynamic spin susceptibility has been obtained both, INS measurements and NMR experiments, can be explored. Probed by INS from the fluctuation-dissipation theorem the q-dependent and o-dependent spin structure factor is related to the dynamical susceptibility by S
~ q; !
1 p1
1 Ims
~ q; ! exp
k!
41
On the other hand, the nuclear spin-lattice relaxation rate aT –1 1a (a =k,k), e. g. for a field Ha applied parallel to the c-axis, given by [66] a
T1k T
1
1 kB 1 Xa 2 Ims
~ q; ! F?
~ q lim 2 2 B k !!0 N q~ k!
42
4 on = 2 np/b [om = (2 m + 1) p/b] denote the fermionic [bosonic] Matsubara frequencies.
105
7
Slave-Boson Approach to Strongly Correlated Electron Systems
and the transverse spin-spin relaxation rate, T –1 2G, for the RKKY coupling of the nuclear Cu spins, given by [67] 2
T2G2
0 12 3 X X 2 c @1 41 2 Fk2
~ qs
~ q F 2
~ qs
~ qA 5 ; N q~ k 8k
2B 4 N q~
43
provide local, atomic site (a = {63, 17} specific information. Here mB denotes the Bohr magneton and the constant c = 0.69 is the natural-abundance fraction of the 63Cu isotope. The form factors are given for 63Cu and the planar 17O nucleus as [68] 63
F
~ q A 2B
cos qx cos qy ;
44
17
F
~ q 2C cos
qx : 2
45
Together with the anisotropy of the Cu relaxation rates the measurements of the Knight shift, a K B a2 n k limq~!0 a F
~ qs
~ q; ! 0, have been used to determine the hyperfine coupling constants Aa, B and C on the basis of the Mila-Rice Hamiltonian [69]. Following Ref. [66] we take A|| & –4B, Ak& 0.84B, C & 0.87B and B & 3.3610–7 eV, where 63 gk = 7.5610 –24 erg/G and 17gk = 3.8610 –24 erg/G. As we know, the RPA susceptibility contains an unphysical instability of the paramagnetic phase at some particular wave-vector q~ below a critical doping dc as signaled by the zero in the denominator of Eq. 39 at o = 0 (Stoner condition). Therefore the use of Eq. 39 only makes sense if the system is far from the magnetic instability, i. e., d > dc , where for J = 0.4 we have dc (t'/t = –0.16) H 0.27 and dc (–0.4) H dc (0) H 0.17.
7.3.3 Inelastic neutron scattering measurements We begin with a discussion of the RPA dynamical spin structure factor S (~ q; o. The q~dependence of S (~ q; o along the main symmetry axis of the Brillouin zone is shown in Fig. 7.9 at J = 0.4 and hole density d = 0.3 for different ratios t'/t. Here the temperature is T = 35 K and the frequency ko = 0.010 eV. For LSCO-type parameters (t'/t = 0, –0.16) we found four pronounced incommensurate peaks located at the points p (1+qo, 1), p (1,1+qo). The incommensurate modulation wave-vectors move with increasing doping level d away from the corner of the Brillouin zone along the directions (1, p) or (p, 1) (square lattice notation). Note, that the incommensurate peak position obtained from a three-band RPA calculation of S (~ q; o [5] can be parametrized consistent with the experimental observation that q0 H 2 x [37], while all the effective one-band RPA approaches [6, 10] yield an incommensurability scaling rather as q0 H d. A more detailed investigation of the LSCO-type q~-scans show that the q~-variation of S (~ q; o is mainly governed by that of w o
~ q; o and, in accordance with experiments [70], the in106
7.3 Comparison with experiments commensurate peaks considerably broaden when temperature or energy transfer are increased [71]. By contrast, the same plot for YBCO-type (t'/t = –0.4) parameters shows a broad and nearly T-independent [71] maximum around the (p, p)-point [72] (Fig. 7.9) which, due to the flat topology of w o , mainly reflects the q~-dependence J (~ q) = J (cosqx + cosqy) (cf. Eq. 39). In this way, our calculations confirm recent arguments [5, 6, 73] for the importance of band structure (Fermi surface geometry) effects in explaining the difference between observed LSCO and YBCO spin dynamics. Nevertheless, whether the incommensurate signals arise from an intrinsic magnetic structure or whether they result from the formation of domains (charge superstructures) in the LSCO system remains unanswered by INS [2, 68].
Figure 7.9: Dynamic magnetic structure factor S (~ q; o is plotted along the (1,1) and (1, p)-directions of the Brillouin zone for different ratios t'/t.
In a next step, we calculate the longitudinal or spin-lattice relaxation rate, T –1 1 , using the hyperfine form factors (Eq. 45). In Figure 7.10 the temperature dependences of 63T –1 1k and 17 –1 T 1k (inset) are shown for d = 0.35 and t'/t = –0.4 in comparison to experiments [74] on fully oxygenated YBCO materials (x = 1). Although our theory does not succeed in giving the correct amplitude of aT –1 1k the qualitative features of the NMR data are described surprisingly well. Obviously, the broad magnetic peak in S (~ q; o at the AFM wave-vector Q~AFM = (p, p) strongly enhances the relaxation rate on Cu sites while, due to a geometrical cancellation (17Fa (~ q Q~AFM 0, the corresponding oxygen rate is rather insensitive to nearly commensurate AFM fluctuations and therefore is governed by the long wavelength part q~ 0 of the spin susceptibility [2]. For 63Cu the nominal Korringa ratio S : (1/T1TK2S) (KS denotes the spin part of the Knight shift) is at least one order of magnitude larger. As can be seen from Fig. 7.10, for YBa2Cu3O7-type parameters, a Korringa (1/T1 ! T ) dependence (dotted line) holds at both Cu and O sites below T* ~ 120K, demonstrating the existence of a characteristic temperature T* as well as in all other near-optimum Tc compounds [2, 75]. T* is in good agreement with the coherence energy scale suggested experimentally [75]. Above T* the 17O NMR relaxation remains linear whereas the 63Cu relaxation time does not follow the Korringa law. 107
7
Slave-Boson Approach to Strongly Correlated Electron Systems
17 –1 Figure 7.10: Spin-lattice relaxation rates 63T –1 T 1k (inset) as a function of temperature. SB results 1k and ((+); t'/t = –0.4, d = 0.35) are compared with experiments (D) on YBa2Cu3O7 [74].
In the oxygen-deficient compound YBa2Cu3O6.6, 1/(63T1kT) shows a broad maximum at about 150 K (Fig. 7.11), which reflects a strong deviation from the canonical Korringa behaviour. In the normal-state regime the theoretical results agree even quantitatively with the experimental 63Cu NMR data [76]. At this point it is important to stress that the present theory incorporates considerable band renormalization effects already via w 0
~ q; o, especially at low doping level. Thus a rather moderate strength J = 0.4 of the AFM exchange interaction yields the experimentally observed enhancement of 63T1k . In striking contrast to the optimally doped YBCO system, the Korringa relation is no longer satisfied for the planar 17O nucleus sites in the underdoped material (cf. inset Fig. 7.11). Instead, a different behaviour 17 T1kT 17 KS = const was suggested to hold down to Tc [76]. The unconventional T-scaling of 17 T1k has been taken as a signature for another important feature of the normal-state spin dynamics, the so-called spin-gap behaviour [2].
Figure 7.11: 63Cu and planar 17O relaxation data (^) for underdoped YBa2Cu3O6.6 [76] are plotted vs temperature. Theoretical results (6) are given at t'/t = –0.4, and d = 0.2.
108
7.4
Summary
Complementary measurements of the transverse spin-spin relaxation rate, T –1 2G , have provided further insights into the drastic change in the magnetic properties when passing from the overdoped to the underdoped regime [67, 77]. As experimentally observed, we found that T –1 2G increases (decreases) with increasing (decreasing) hole doping (temperature) [78]. In order to detect the opening of a spin-pseudogap as a function of T, a powerful technique is to measure the ratio T2G /T1T [79] which is nearly constant above ~ 200 K for deoxygenated YBa2Cu3O6.6 [67]. The calculated temperature dependence of this quantity is shown in Fig. 7.12 together with recent experimental results [67]. Most notably, the opening of a spin-pseudo gap at T* ~ 135 K [79], i. e. well above Tc, is clearly seen as a decrease of below T*. Note that for YBa2Cu3O7, as predicted by Fermi liquid theories, the ratio T22G /T1T is approximately constant above 150 K [2].
Figure 7.12: T2G /(63T1kT ) in YBa2Cu3O6.6 (^) as measured by Takigawa [67] compared with the SB data (6) at t'/t = –0.4, and d = 0.2.
7.4
Summary
In this work we have used a spin-rotation-invariant SB approach to investigate magnetic and transport properties of the 2D t-t'-J model. Our main results are the following (see also [81]): a) We present a detailed magnetic ground-state phase diagram of the 2D t-(t')-Jmodel, including incommensurate magnetic structures and phase separated states. At finite t', a main feature of the phase diagram, we would like to emphasize, is the existence of an AFM state away from half-filling, which is locally and also globally stable against phase separation. This result agrees with the experimentally observed AFM long-range order in the weakly doped LSCO and YBCO compounds. In contrast, for the simple t-J model we observe no AFM long-range order at any finite doping due to phase separation. 109
7
Slave-Boson Approach to Strongly Correlated Electron Systems
b) The next nearest-neighbour hopping process (t') incorporates important correlation and band structure effects near half-filling. In particular, the t'-term can be used to reproduce the FS geometry of LSCO, YBCO, and NCCO. Also the NNN hopping provides a possible origin for the experimentally observed asymmetry in the persistence of AFM order of holedoped and electron-doped systems. c) The quality of the SRI SB approach was demonstrated in comparison with exact diagonalization results available for the t-J model on finite square lattices with up to 36 sites. In this case, the SB method yields an excellent estimate for the quasi-particle band renormalization. d) Within the saddle-point and relaxation time approximation, our SB calculation of the Hall resistivity in the t-t'-J model provides a reasonable explanation of the experimentally observed doping dependence of RH on both hole-doped (La2–xSrxCuO4, YBa2Cu3O6+x) and electron-doped (Nd2–xCexCuO4) copper oxides. e) Using a generalized RPA expression for the spin susceptibility and assuming that the AFM correlations are spatially filtered by the hyperfine form factors, we have calculated the temperature dependences of spin-lattice and spin-spin relaxation rates for planar copper and oxygen sites. The results agree qualitatively well with various NMR experiments on YBa2Cu3O6+x. In addition, we can attribute the contrasting q~-dependence of the magnetic structure factor S (~ q; o seen in INS experiments for LSCO-type and YBCO-type systems to differences in their fermiology. Recently, our theory was improved to include (Gaussian) fluctuations beyond the paramagnetic saddle-point approximation [27, 80]. We derived a concise expression for the spin susceptibility ws (~ q; o of the t-t '-J model which does not have the standard RPA form. Then we were able to show that the instability line obtained from a divergence of ws (~ q; 0 is in agreement with the PM ⇔ spiral state phase boundary in the saddle-point phase diagram, which in fact proves the consistency of both approaches [27].
References
1. For a recent overview of the experimental and theoretical situation see: Proceedings of the Int. Conf. M2S HTSC IV, Grenoble 1994, in: Physica C, 235–240 (1994) Proceedings of the Int. Euroconf. on Magnetic Correlations, Metal-Insulator-Transitions, and Superconductivity in Novel Materials, Würzburg 1994, in: J. Low. Temp. Phys., 3/4 (1995) 2. A.P. Kampf: Physics Reports, 249, 219 (1994) 3. A.J. Millis, H. Monien: Phys., Rev. Lett. 70, 2810 (1993) 4. P. Monthoux, D. Pines: Phys. Rev. B, 49, 4261 (1941) 5. Q. Si, Y. Zha, K. Levin, J.P. Lu: Phys. Rev. B, 47, 9055 (1993) 6. T. Tanamoto, K. Kuboki, H. Fukuyama: J. Phys. Soc. Jpn., 60, 3072 (1991) T. Tanamoto, H. Kohno, H. Fukuyama: J. Phys. Soc. Jpn., 62, 717 (1993)
110
References
7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30. 31. 32. 33. 34. 35. 36. 37. 38. 39. 40. 41. 42. 43. 44. 45. 46. 47. 48. 49. 50. 51. 52. 53. 54. 55. 56.
T. Tanamoto, H. Kohno, H. Fukuyama: J. Phys. Soc. Jpn., 62, 1455 (1993) T. Tanamoto, H. Kohno, H. Fukuyama: J. Phys. Soc. Jpn., 63, 2739 (1994) T. Ito, K. Takenaka, S. Uchida: Phys. Rev. Lett., 70, 3995 (1993) V.J. Emery: Phys. Rev. Lett., 58, 2794 (1987) M.S. Hybertsen, M. Schlüter, N. E. Christensen: Phys. Rev. B, 39, 9028 (1989) P. Bénard, L. Chen, A.-M. S. Tremblay: Phys. Rev. B, 47, 15 217 (1993) M. Lavagna, G. Stemmann: Phys. Rev. B, 49, 4235 (1994) T. Tohyama, S. Maekawa: Phys. Rev. B, 49, 3596 (1994) J. Yu, S. Massida, A.J. Freeman: Phys. Lett. A, 122, 198 (1987) D.M. King et al: Phys. Rev. Lett., 70, 3159 (1993) P.A. Lee: Phys. Rev. Lett., 63, 680 (1989) D.M. News, M. Rasolt, P. Pattnik: Phys. Rev. B, 38, 6513 (1988) Z. Zou, P.W. Anderson: Phys. Rev. B, 37, 627 (1988) D. Yoshioka: J. Phys. Soc. Jpn., 58, 1516 (1989) H. Kaga: Phys. Rev. B, 46, 1979 (1992) S.K. Sarker: Phys. Rev. B, 47, 2940 (1993) J. Igarashi, P. Fulde: Phys. Rev. B, 48, 998 (1993) Y.M. Li, D.N. Sheng, Z. B. Su, L. Yu: Phys. Rev. B, 45, 5428 (1992) S.D. Liang, B. Doucot, P.W. Anderson: Phys. Rev. Lett., 61, 365 (1988) G. Kotliar, A.E. Ruckenstein: Phys. Rev. Lett., 57, 1362 (1986) R. Frésard, P. Wölfle: Int. J. Mod. Phys. B, 5&6, 685; Erratum ibid. 3087 (1992) M. Deeg, H. Fehske, H. Büttner: Europhys. Lett., 26, 109 (1994) M. Deeg, H. Fehske: Phys. Rev. B, 50, 17 874 (1994) T. Li, P. Wölfle, P.J. Hirschfeld: Phys. Rev. B, 40, 6817 (1989) J.W. Negele, H. Orland: Quantum Many-Particle Systems, Addison-Wesley, Reading, MA (1988) T. Jolicoeur, J.C.L. Guillou: Phys. Rev. B, 44, 2403 (1991) E. Arrigoni et al.: Physics Reports, 241, 291 (1994) M. Deeg, H. Fehske, H. Büttner: Z. Phys. B, 88, 283 (1992) L. Lilly, A. Muramatsu, W. Hanke: Phys. Rev. Lett., 65, 1379 (1990) R. Frésard, M. Dzierzawa, P. Wölfle: Europhys. Lett., 15, 325 (1991) E. Arrigoni, G.C. Strinati: Phys. Rev. B, 44, 7455 (1991) B. Möller, K. Doll, R. Frésard: J. Phys. Condens. Matter, 5, 4847 (1993) D. Boies, F.A. Jackson, A.-M.S. Tremblay: Int. J. Mod. Phys. B, 9, 1001 (1995) S.-W. Cheong et al.: Phys. Rev. Lett., 67, 1791 (1991) G.C. Psaltakis, N. Papanicolaou: Phys. Rev. B, 48, 456 (1993) H. Mori, M. Hamada: Phys. Rev. B, 48, 6242 (1993) A.P. Kampf, W. Brenig: J. Low Temp. Phys,. 95, 335 (1994) V. Chechersky et al.: Phys. Rev. Lett., 70, 3355 (1993) M. Matsuda et al.: Phys. Rev. B, 45, 12 548 (1992) G.M. Luke et al.: Phys. Rev. B, 42, 7981 (1990) T.R. Thurston et al.: Phys. Rev. B, 40, 4585 (1990) J. Rossat-Mignod et al.: Physica B, 180 & 181, 383 (1992) V.J. Emery, S. A. Kivelson: Physica C, 209, 597 (1993) V.J. Emery, S. A. Kivelson, H. Q. Lin: Phys. Rev. Lett., 64, 475 (1990) H. Fehske, V. Waas, H. Röder, H. Büttner: Phys. Rev., B 44, 8473 (1991) M. Marder, N. Papanicolaou, G. C. Psaltakis: Phys. Rev. B, 41, 6920 (1990) E.V.L. de Mello: J. Phys. Condens. Matter, 6, 117 (1994) W.O. Puttika, M. Luchini, T.M. Rice: Phys. Rev. Lett., 68, 538 (1992) V. Waas, H. Fehske, H. Büttner: Phys. Rev. B, 48, 9106 (1993) H. Takagi et al.: Phys. Rev. B, 40, 2254 (1989) E.C. Jones et al.: Phys. Rev. B, 47, 8986 (1993) H. Takagi, S. Uchida, Y. Tokura: Phys. Rev. Lett., 62, 1197 (1989) S.J. Hagen, J.L. Peng, Z.Y. Li, R.L. Greene: Phys. Rev. B, 43, 13 606 (1991)
111
7 57. 58. 59. 60. 61. 62. 63. 64. 65. 66. 67. 68. 69. 70. 71. 72. 73. 74. 75. 76. 77. 78. 79. 80. 81.
112
Slave-Boson Approach to Strongly Correlated Electron Systems
H. Takagi et al.: Phys. Rev. Lett., 69, 2975 (1992) J.C. Campuzano et al.: Phys. Rev., Lett. 64, 2308 (1990) W.E. Pickett: Rev. Mod. Phys., 61, 433 (1989) S.A. Trugman: Phys. Rev. Lett., 65, 500 (1990) H. Chi, A.D.S. Nagi: Phys. Rev. B, 46, 421 (1992) H. Fehske, M. Deeg: Solid State Commun., 93, 41 (1995) E. Dagotto, A. Nazarenko, M. Bonsinsegni, Phys. Rev. Lett., 73, 728 (1994) S. Sarker, C. Jayaprakash, H.R. Krishnamurthy, W. Wenzel: Phys. Rev. B, 43, 8775 (1991) R. Grempel, M. Lavagna: Solid State Commun., 83, 595 (1992) H. Monien, P. Monthoux, D. Pines: Phys. Rev. B, 42, 167 (1990) M. Takigawa: Phys. Rev. B, 49, 4158 (1994) V. Barzykin, D. Pines, D. Thelen: Phys. Rev. B, 50, 16 052 (1994) F. Mila, T.M. Rice: Physica C, 157, 561 (1989) T.E. Mason, G. Aeppli, H.A. Mook: Phys. Rev. Lett., 68, 1414 (1992) H. Fehske, M. Deeg: J. Low. Temp. Phys., 3/4, 425 (1995) J. Rossat-Mignod et al.: Physica C, 185–189, 86 (1991) P. Littlewood, J. Zaanen, G. Aeppli, H. Monien: Phys. Rev. B, 48, 487 (1993) M. Takigawa et al.: Physica C, 162, 853 (1989) P.C. Hammel et al.: Phys. Rev. Lett., 63, 1992 (1989) M. Takigawa et al.: Phys. Rev. B, 43, 247 (1991) Y. Itoh et al.: J. Phys. Soc. Jpn., 61, 1287 (1992) M. Deeg: PhD thesis, Universität Bayreuth, (1995) C. Berthier et al.: Physica C, 235–240, 67 (1994) M. Deeg et al., Z. Phys. B, 95, 87 (1994) H. Fehske, Spin Dynamics, Charge Transport, and Electron-Phonon Coupling Effects in Strongly Correlated Electron Systems, Habilitationsschrift, Universität Bayreuth (1995)
8
Non-Linear Excitations and the Electronic Structure of Conjugated Polym