Advanced MEMS Packaging
This page intentionally left blank
Advanced MEMS Packaging John H. Lau Chengkuo Lee C. S. Premachandran Yu Aibin
New York Chicago San Francisco Lisbon London Madrid Mexico City Milan New Delhi San Juan Seoul Singapore Sydney Toronto
Copyright © 2010 by The McGraw-Hill Companies, Inc. All rights reserved. Except as permitted under the United States Copyright Act of 1976, no part of this publication may be reproduced or distributed in any form or by any means, or stored in a database or retrieval system, without the prior written permission of the publisher. ISBN: 978-0-07-162792-4 MHID: 0-07-162792-8 The material in this eBook also appears in the print version of this title: ISBN: 978-0-07-162623-1, MHID: 0-07-162623-9. All trademarks are trademarks of their respective owners. Rather than put a trademark symbol after every occurrence of a trademarked name, we use names in an editorial fashion only, and to the benefit of the trademark owner, with no intention of infringement of the trademark. Where such designations appear in this book, they have been printed with initial caps. McGraw-Hill eBooks are available at special quantity discounts to use as premiums and sales promotions, or for use in corporate training programs. To contact a representative please e-mail us at
[email protected]. Information contained in this work has been obtained by The McGraw-Hill Companies, Inc. (“McGraw-Hill”) from sources believed to be reliable. However, neither McGraw-Hill nor its authors guarantee the accuracy or completeness of any information published herein, and neither McGraw-Hill nor its authors shall be responsible for any errors, omissions, or damages arising out of use of this information. This work is published with the understanding that McGraw-Hill and its authors are supplying information but are not attempting to render engineering or other professional services. If such services are required, the assistance of an appropriate professional should be sought. TERMS OF USE This is a copyrighted work and The McGraw-Hill Companies, Inc. (“McGraw-Hill”) and its licensors reserve all rights in and to the work. Use of this work is subject to these terms. Except as permitted under the Copyright Act of 1976 and the right to store and retrieve one copy of the work, you may not decompile, disassemble, reverse engineer, reproduce, modify, create derivative works based upon, transmit, distribute, disseminate, sell, publish or sublicense the work or any part of it without McGraw-Hill’s prior consent. You may use the work for your own noncommercial and personal use; any other use of the work is strictly prohibited. Your right to use the work may be terminated if you fail to comply with these terms. THE WORK IS PROVIDED “AS IS.” McGRAW-HILL AND ITS LICENSORS MAKE NO GUARANTEES OR WARRANTIES AS TO THE ACCURACY, ADEQUACY OR COMPLETENESS OF OR RESULTS TO BE OBTAINED FROM USING THE WORK, INCLUDING ANY INFORMATION THAT CAN BE ACCESSED THROUGH THE WORK VIA HYPERLINK OR OTHERWISE, AND EXPRESSLY DISCLAIM ANY WARRANTY, EXPRESS OR IMPLIED, INCLUDING BUT NOT LIMITED TO IMPLIED WARRANTIES OF MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. McGraw-Hill and its licensors do not warrant or guarantee that the functions contained in the work will meet your requirements or that its operation will be uninterrupted or error free. Neither McGraw-Hill nor its licensors shall be liable to you or anyone else for any inaccuracy, error or omission, regardless of cause, in the work or for any damages resulting therefrom. McGraw-Hill has no responsibility for the content of any information accessed through the work. Under no circumstances shall McGraw-Hill and/or its licensors be liable for any indirect, incidental, special, punitive, consequential or similar damages that result from the use of or inability to use the work, even if any of them has been advised of the possibility of such damages. This limitation of liability shall apply to any claim or cause whatsoever whether such claim or cause arises in contract, tort or otherwise.
About the Authors John H. Lau earned a Ph.D. in theoretical and applied mechanics from the University of Illinois. He has also earned three master’s degrees. He currently is a visiting professor at the Hong Kong University of Science & Technology (HKUST). His research interests cover a broad range of enabling technologies for 3D IC and system-in-package integration for RoHS-compliant electronics, optoelectronics, photonics, and MEMS packaging. Prior to joining HKUST, Dr. Lau was the director of the Microsystems, Modules, and Components Laboratory at the Institute of Microelectronics in Singapore for 2 years and a Senior Scientist/MTS at Agilent/Hewlett-Packard in California for more than 25 years. With more than 35 years of R&D and manufacturing experience, he has authored or co-authored more than 400 peer-reviewed technical publications, books, book chapters, and papers. Dr. Lau has received awards from ASME and IEEE, and is a Fellow of both organizations. Chengkuo Lee received a Ph.D. in precision engineering from the University of Tokyo, and has also earned two master’s degrees. He worked as a researcher in several labs and then managed the MEMS device division at the Metrodyne Microsystem Corporation in Taiwan. Dr. Lee co-founded Asia Pacific Microsystems, Inc., in Taiwan, and served as vice president. He is now an assistant professor in the Department of Electrical and Computer Engineering at National University of Singapore and a senior member of the technical staff at the Institute of Microelectronics in Singapore. He has authored or co-authored about 200 conference papers, extended abstracts, and peer-reviewed journal articles, and holds eight U.S. patents in the MEMS and nanotechnology fields. C. S. Premachandran earned a master of technology degree in solid state technology from the Indian Institute of Technology, Madras. He has held managerial/ executive positions at Indian Telephone Industries, Sun Fiber Optics, and Delphi Automotive Systems. Since 1998 he has worked as a member of the technical staff in
the Microsystems, Modules, and Components Laboratory at the Institute of Microelectronics, Singapore. He has authored or co-authored more than 50 conference papers and journal articles and holds 10 U.S. patents. He is a Senior Member of IEEE. His research interests are in MEMS and biosensor, optical, and advanced packaging. Yu Aibin received a Ph.D. in electrical and electronic engineering from Nanyang Technological University in Singapore. He is a senior research engineer in the Microsystems, Modules, and Components Laboratory at the Institute of Microelectronics in Singapore. His research interests include advanced packaging and MEMS design, fabrication, and packaging. Dr. Yu has authored or co-authored more than 60 technical publications.
Contents Foreword . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . xv Preface . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . xvii Acknowledgments . . . . . . . . . . . . . . . . . . . . . . . . . . . xxi 1
2
3
Introduction to MEMS . . . . . . . . . . . . . . . . . . . . . . . . 1.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 1.2 Commercial Applications of MEMS . . . . . . . . 1.3 MEMS Markets . . . . . . . . . . . . . . . . . . . . . . . . . 1.4 Top 30 MEMS Suppliers . . . . . . . . . . . . . . . . . . 1.5 Introduction to MEMS Packaging . . . . . . . . . . 1.6 MEMS Packaging Patents since 2001 . . . . . . . 1.6.1 U.S. MEMS Packaging Patents . . . . . 1.6.2 Japanese MEMS Packaging Patents . . . 1.6.3 Worldwide MEMS Packaging Patents . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
1 1 2 2 5 5 6 6 21
Advanced MEMS Packaging . . . . . . . . . . . . . . . . . . . 2.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 2.2 Advanced IC Packaging . . . . . . . . . . . . . . . . . . 2.2.1 Moore’s Law versus More Than Moore (MTM) . . . . . . . . . . . . . . . . . . . 2.2.2 3D IC Integration with WLP . . . . . . . 2.2.3 Low-Cost Solder Microbumps for 3D IC SiP . . . . . . . . . . . . . . . . . . . . 2.2.4 Thermal Management of 3D IC SiP with TSV ....................... 2.3 Advanced MEMS Packaging . . . . . . . . . . . . . . 2.3.1 3D MEMS WLP: Designs and Materials . . . . . . . . . . . . . . . . . . . . . . . . 2.3.2 3D MEMS WLP: Processes . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
47 47 47
Enabling Technologies for Advanced MEMS Packaging . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 3.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 3.2 TSVs for MEMS Packaging . . . . . . . . . . . . . . . 3.2.1 Via Formation . . . . . . . . . . . . . . . . . . . 3.2.2 Dielectric Isolation Layer (SiO2) Deposition . . . . . . . . . . . . . . . . . . . . . .
27 43
47 49 52 58 67 68 72 76 81 81 81 82 86
vii
viii
Contents 3.2.3
3.3
3.4
3.5
3.6
3.7
Barrier/Adhesion and Seed Metal Layer Deposition . . . . . . . . . . . . . . . . . 3.2.4 Via Filling . . . . . . . . . . . . . . . . . . . . . . . 3.2.5 Cu Polishing by Chemical/ Mechanical Polish (CMP) . . . . . . . . . 3.2.6 Fabrication of an ASIC Wafer with TSVs ...................... 3.2.7 Fabrication of Cap Wafer with TSVs and Cavity . . . . . . . . . . . . . . . . . Piezoresistive Stress Sensors for MEMS Packaging . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 3.3.1 Design and Fabrication of Piezoresistive Stress Sensors . . . . . . . 3.3.2 Calibration of Stress Sensors . . . . . . . 3.3.3 Stresses in Wafers after Mounting on a Dicing Tape . . . . . . . . . . . . . . . . . 3.3.4 Stresses in Wafers after Thinning (Back-Grinding) . . . . . . . . . . . . . . . . . . Wafer Thinning and Thin-Wafer Handling . . . . 3.4.1 3M Wafer Support System . . . . . . . . . 3.4.2 EVG’s Temporary Bonding and Debonding System . . . . . . . . . . . . . . . 3.4.3 A Simple Support-Wafer Method for Thin-Wafer Handling . . . . . . . . . . . . . Low-Temperature Bonding for MEMS Packaging . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 3.5.1 How Does Low-Temperature Bonding with Solders Work? . . . . . . . . . . . . . . . 3.5.2 Low-Temperature C2C Bonding . . . . 3.5.3 Low-Temperature C2W Bonding . . . 3.5.4 Low-Temperature W2W Bonding . . . . MEMS Wafer Dicing . . . . . . . . . . . . . . . . . . . . . 3.6.1 Fundamentals of SD Technology . . . 3.6.2 Dicing of SOI Wafers . . . . . . . . . . . . . 3.6.3 Dicing of Silicon-on-Silicon Wafers . . . 3.6.4 Dicing of Silicon-on-Glass Wafers . . . RoHS-Compliant MEMS Packaging . . . . . . . . 3.7.1 EU RoHS . . . . . . . . . . . . . . . . . . . . . . . . 3.7.2 What Is the Definition of X-Free (e.g., Pb-Free)? .................. 3.7.3 What Is a Homogeneous Material? . . . . . . . . . . . . . . . . . . . . . . . . 3.7.4 What Is the TAC? . . . . . . . . . . . . . . . . 3.7.5 How Is a Law Published in the EU RoHS Directive? . . . . . . . . . . . . . . . . .
87 89 91 92 93 93 93 95 98 101 104 104 105 108 111 112 113 122 124 126 126 129 130 130 133 133 134 134 135 135
Contents 3.7.6 3.7.7 3.7.8 References 4
5
EU RoHS Exemptions . . . . . . . . . . . . Current Status of RoHS Compliance in the Electronics Industry . . . . . . . . . Lead-Free Solder-Joint Reliability of MEMS Packages . . . . . . . . . . . . . . . . . ..................................
Advanced MEMS Wafer-Level Packaging . . . . . . . 4.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 4.2 Micromachining, Wafer-Bonding Technologies, and Interconnects . . . . . . . . . . . 4.2.1 Thin-Film Technologies . . . . . . . . . . . 4.2.2 Bulk Micromachining Technologies . . . . . . . . . . . . . . . . . . . . 4.2.3 Conventional Wafer-Bonding Technologies for Packaging . . . . . . . . 4.2.4 Plasma-Assisted Wafer-Bonding Technologies . . . . . . . . . . . . . . . . . . . . 4.2.5 Electrical Interconnects . . . . . . . . . . . 4.2.6 Solder-Based Intermediate-Layer Bonding . . . . . . . . . . . . . . . . . . . . . . . . 4.3 Wafer-Level Encapsulation . . . . . . . . . . . . . . . 4.3.1 High-Temperature Encapsulation Process . . . . . . . . . . . . . . . . . . . . . . . . . 4.3.2 Low-Temperature Encapsulation Process . . . . . . . . . . . . . . . . . . . . . . . . . 4.4 Wafer-Level Chip Capping and MCM Technologies . . . . . . . . . . . . . . . . . . . . . . . . . . . . 4.5 Wafer-Level MEMS Packaging Based on Low-Temperature Solders: Case Study . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 4.5.1 Case Study: In/Ag System of Noneutectic Composition . . . . . . . . . 4.5.2 Case Study: Eutectic InSn Solder for Cu-Based Metallization . . . . . . . . . . . 4.6 Summary and Future Outlook . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Optical MEMS Packaging: Communications . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 5.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 5.2 Actuation Mechanisms and Integrated Micromachining Processes . . . . . . . . . . . . . . . . 5.2.1 Electrostatic Actuation . . . . . . . . . . . . 5.2.2 Thermal Actuation . . . . . . . . . . . . . . . 5.2.3 Magnetic Actuation . . . . . . . . . . . . . .
135 138 138 149 157 157 158 158 159 168 172 172 175 176 177 178 180
182 183 193 202 203 209 209 211 212 215 219
ix
x
Contents 5.2.4 5.2.5
Piezoelectric Actuation . . . . . . . . . . . . Integrated Micromachining Processes . . . . . . . . . . . . . . . . . . . . . . . . 5.3 Optical Switches . . . . . . . . . . . . . . . . . . . . . . . . 5.3.1 Small-Scale Optical Switches . . . . . . . 5.3.2 Large-Scale Optical Switches . . . . . . 5.4 Variable Optical Attenuators . . . . . . . . . . . . . . 5.4.1 Early Development Work . . . . . . . . . 5.4.2 Surface-Micromachined VOAs . . . . . 5.4.3 DRIE-Derived Planar VOAs Using Electrostatic Actuators . . . . . . . . . . . . 5.4.4 DRIE-Derived Planar VOAs Using Electrothermal (Thermal) Actuators . . . . . . . . . . . . . . . . . . . . . . . 5.4.5 3D VOAs . . . . . . . . . . . . . . . . . . . . . . . 5.4.6 VOAs Using Various Mechanisms . . . . . . . . . . . . . . . . . . . . . 5.5 Packaging, Testing, and Reliability Issues . . . . 5.5.1 Manufacturability and Self-Assembly . . . . . . . . . . . . . . . . . . . 5.5.2 Case Study: VOAs . . . . . . . . . . . . . . . . 5.5.3 Case Study: Optical Switches . . . . . . 5.6 Summary and Future Outlook . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 6
Optical MEMS Packaging: Bubble Switch . . . . . . . 6.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 6.2 3D Packaging . . . . . . . . . . . . . . . . . . . . . . . . . . . 6.3 Boundary-Value Problem . . . . . . . . . . . . . . . . . 6.3.1 Geometry . . . . . . . . . . . . . . . . . . . . . . . 6.3.2 Materials . . . . . . . . . . . . . . . . . . . . . . . . 6.3.3 Boundary Conditions . . . . . . . . . . . . . 6.4 Nonlinear Analyses of the 3D Photonic Switch . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 6.4.1 Creep Hysteresis Loops . . . . . . . . . . . 6.4.2 Deflections . . . . . . . . . . . . . . . . . . . . . . 6.4.3 Shear-Stress Time-History . . . . . . . . . 6.4.4 Shear-Creep-Strain Time-History . . . 6.4.5 Creep-Strain Energy-Density Range . . . . 6.5 Isothermal Fatigue Tests and Results . . . . . . . 6.5.1 Sample Preparation . . . . . . . . . . . . . . 6.5.2 Test Setup and Procedures . . . . . . . . . 6.5.3 Test Results . . . . . . . . . . . . . . . . . . . . . 6.6 Thermal Fatigue Life Prediction of the Sealing Ring . . . . . . . . . . . . . . . . . . . . . . . . . . . .
219 221 224 225 233 237 238 240 242
252 254 258 261 264 269 275 285 286 297 297 297 302 302 302 305 306 306 307 307 307 308 309 309 309 312 314
Contents 6.7 Appendix A: Package Deflection by Twyman-Green Interferometry Method . . . . 6.7.1 Sample Preparation . . . . . . . . . . . . . . 6.7.2 Test Setup and Procedure . . . . . . . . . 6.7.3 Temperature Conditions . . . . . . . . . . 6.7.4 Measurement Results . . . . . . . . . . . . . 6.8 Appendix B: Package Deflection by Finite-Element Method . . . . . . . . . . . . . . . . . . . 6.9 Appendix C: Finite-Element Modeling of the Bolt . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 6.9.1 Description of the Bolted Model . . . . 6.9.2 Responses of the Bolted Photonic Switch . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 7
8
Optical MEMS: Microbolometer Packaging ..... 7.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 7.2 Bolometer Chip . . . . . . . . . . . . . . . . . . . . . . . . . 7.3 Thermal Optimization . . . . . . . . . . . . . . . . . . . 7.3.1 Final Temperature Stability Testing . . . . . . . . . . . . . . . . . . . . . . . . . . 7.4 Structural Optimization of the Package .... 7.5 Vacuum Packaging of Bolometer . . . . . . . . . . 7.5.1 Ge Window . . . . . . . . . . . . . . . . . . . . . 7.6 Getter Attachment and Activation . . . . . . . . . 7.7 Outgassing Study in a Vacuum Package . . . . 7.8 Testing Setup for Bolometer . . . . . . . . . . . . . . . 7.8.1 Package Testing . . . . . . . . . . . . . . . . . . 7.8.2 Image Testing . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Bio-MEMS Packaging . . . . . . . . . . . . . . . . . . . . . . . . . 8.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 8.2 Bio-MEMS Chip ........................ 8.3 Microfluidic Components . . . . . . . . . . . . . . . . 8.3.1 Microfluidic Cartridge . . . . . . . . . . . . 8.3.2 Biocompatible Polymeric Materials . . . . . . . . . . . . . . . . . . . . . . . . 8.4 Microfluidic Packaging .................. 8.4.1 Polymer Microfabrication Techniques . . . . . . . . . . . . . . . . . . . . . . 8.4.2 Replication Technologies . . . . . . . . . . 8.4.3 Overview of Existing DNA and RNA Extractor Biocartridges . . . . . . . 8.5 Fabrication of PDMS Layers . . . . . . . . . . . . . . 8.6 Assembly of PDMS Microfluidic Packages . . .
314 315 316 317 317 317 320 320 322 325 327 327 329 330 334 335 340 342 344 346 347 347 350 352 353 353 355 357 357 359 362 362 362 363 364 364
xi
xii
Contents 8.6.1
Microfluidic Package without Reservoirs . . . . . . . . . . . . . . . . . . . . . . . 8.6.2 Development of Reservoir and Valve . . . . . . . . . . . . . . . . . . . . . . . 8.7 Self-Contained Microfluidic Cartridge ..... 8.7.1 Microfluidic Package with Self-Contained Reservoirs . . . . . . . . . 8.7.2 Pin-Valve Design . . . . . . . . . . . . . . . . . 8.7.3 Fluid Flow-Control Mechanism . . . . 8.8 Fabrication . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 8.8.1 Substrate Fabrication . . . . . . . . . . . . . 8.8.2 Material Selection for the Reservoir Membrane . . . . . . . . . . . . . . . . . . . . . . 8.9 Permeability of Material . . . . . . . . . . . . . . . . . . 8.10 Thermocompression Bonding . . . . . . . . . . . . . 8.10.1 Bonding of PMMA to PMMA for the Channel Layer . . . . . . . . . . . . . . . . . . . 8.10.2 Polypropylene to PMMA for Reservoir and Channel Layer . . . . . . 8.10.3 Tensile Test . . . . . . . . . . . . . . . . . . . . . . 8.11 Microfluidic Package Testing . . . . . . . . . . . . . . 8.11.1 Fluid Testing . . . . . . . . . . . . . . . . . . . . 8.11.2 Biologic Testing on a Biosample . . . . 8.12 Sample Preparation and Setup . . . . . . . . . . . . 8.12.1 Pretreatment of the Cartridge ..... 8.12.2 PCR Amplification . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 9
Biosensor Packaging . . . . . . . . . . . . . . . . . . . . . . . . . . 9.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 9.1.1 Review of Optical Coherence Tomography (OCT) . . . . . . . . . . . . . . 9.2 Biosensor Packaging .................... 9.2.1 Micromirror . . . . . . . . . . . . . . . . . . . . . 9.2.2 Single-Mode Optical Fiber and GRIN Lens . . . . . . . . . . . . . . . . . . . . . . . . . . . . 9.2.3 Upper Substrate . . . . . . . . . . . . . . . . . 9.2.4 Lower Substrate . . . . . . . . . . . . . . . . . 9.3 The Package . . . . . . . . . . . . . . . . . . . . . . . . . . . . 9.3.1 Configuration of the Probe . . . . . . . . 9.3.2 Optical Properties and Theories ... 9.3.3 Evaluations of Parameters . . . . . . . . . 9.4 Optical Simulation . . . . . . . . . . . . . . . . . . . . . . . 9.4.1 Optical Model of the Probe . . . . . . . . 9.4.2 Effect of Mirror Curvature on Coupling Efficiency . . . . . . . . . . . . . .
366 370 371 371 374 375 377 377 381 381 384 385 387 390 391 391 392 394 394 394 395 397 397 398 401 401 401 403 404 404 404 406 410 412 412 415
Contents 9.4.3 Effect of Lateral Tilt of a Flat Micromirror on a Curved Sample . . . . 9.4.4 Effect of Vertical Tilt of a Flat Micromirror on a Curved Sample . . . 9.4.5 Effect of Vertical Tilt of a Flat Micromirror on a Flat Sample . . . . . . 9.5 Assembly of the Optical Probe . . . . . . . . . . . . 9.5.1 Fabrication of SiOB . . . . . . . . . . . . . . . 9.5.2 Probe Assembly . . . . . . . . . . . . . . . . . . 9.5.3 Probe Housing .................. 9.6 Testing of the Probe ..................... 9.6.1 Optical Alignment . . . . . . . . . . . . . . . 9.6.2 Axial Scanning Test Result . . . . . . . . . 9.6.3 Probe Imaging .................. 9.6.4 Optical Efficiency Testing . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 10
11
Accelerometer Packaging . . . . . . . . . . . . . . . . . . . . . . 10.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 10.2 Wafer-Level Package Requirements ....... 10.2.1 Electrical Modeling . . . . . . . . . . . . . . . 10.2.2 Package Structure . . . . . . . . . . . . . . . . 10.2.3 Extraction Methodology of the Interconnection Characteristics . . . . . 10.3 Wafer-Level Packaging Process . . . . . . . . . . . . 10.3.1 Method 1: TSV with Sacrificial Wafer . . . . . . . . . . . . . . . . . . . . . . . . . . . 10.3.2 Method 2: TSV without Sacrificial Wafer . . . . . . . . . . . . . . . . . . . . . . . . . . . 10.3.3 Method 3: TSV with MEMS Wafer . . . . . . . . . . . . . . . . . . . . . . . . . . . 10.4 Wafer Separation Process . . . . . . . . . . . . . . . . . 10.4.1 Process Integration . . . . . . . . . . . . . . . 10.5 Sacrificial Wafer Removal . . . . . . . . . . . . . . . . 10.6 Wafer-Level Vacuum Sealing ............. 10.7 Vacuum Measurement Using a MEMS Motion Analyzer ....................... 10.8 Reliability Testing: Vacuum Maintenance ... 10.9 Wafer-Level 3D Package for an Accelerometer . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Radiofrequency MEMS Switches . . . . . . . . . . . . . . 11.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 11.2 Design of RF MEMS Switches . . . . . . . . . . . . . 11.2.1 Design of Capacitive Switches . . . . .
417 419 420 421 421 422 425 427 427 427 429 431 433 435 435 437 438 438 442 448 450 450 452 458 460 462 464 467 469 471 473 475 475 475 475
xiii
xiv
Contents 11.2.2 Design of Metal-Contact Switches . . . . 11.2.3 Mechanical Design of RF MEMS Switches . . . . . . . . . . . . . . . . . . . . . . . . 11.3 Fabrication of RF MEMS Switches . . . . . . . . . 11.3.1 Surface Micromachining of RF MEMS Switches . . . . . . . . . . . . . . . . . . 11.3.2 Bulk Micromachining of RF MEMS Switches . . . . . . . . . . . . . . . . . . . . . . . . 11.4 Characterization of RF MEMS Switches . . . . 11.4.1 RF Performance . . . . . . . . . . . . . . . . . . 11.4.2 Mechanical Performance . . . . . . . . . . 11.5 Reliability of RF MEMS Switches . . . . . . . . . . 11.5.1 Reliability of Capacitive Switches . . . . . . . . . . . . . . . . . . . . . . . . 11.5.2 Reliability of Metal-Contact Switches . . . . . . . . . . . . . . . . . . . . . . . . 11.6 Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 12
13
RF MEMS Tunable Capacitors and Tunable Band-Pass Filters . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 12.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 12.2 RF MEMS Tunable Capacitors . . . . . . . . . . . . 12.2.1 Analog Tuning of RF MEMS Capacitors . . . . . . . . . . . . . . . . . . . . . . 12.2.2 Digital Tuning of RF MEMS Capacitors . . . . . . . . . . . . . . . . . . . . . . 12.3 RF MEMS Tunable Band-Pass Filters . . . . . . . 12.3.1 Analog Tuning of a MEMS Band-Pass Filter . . . . . . . . . . . . . . . . . . 12.3.2 Digital Tuning of an RF MEMS Filter . . . . . . . . . . . . . . . . . . . . . . . . . . . 12.4 Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
479 479 484 484 488 489 489 489 492 492 492 492 493 495 495 495 496 503 504 505 506 512 513
Advanced Packaging of RF MEMS Devices . . . . . 13.1 Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . 13.2 Zero-Level Packaging . . . . . . . . . . . . . . . . . . . . 13.2.1 Chip Capping . . . . . . . . . . . . . . . . . . . 13.2.2 Thin-Film Capping . . . . . . . . . . . . . . . 13.3 One-Level Packaging . . . . . . . . . . . . . . . . . . . . 13.4 Reliability of Packaged RF MEMS Devices . . . 13.5 Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
515 515 515 516 523 525 526 528 528
Index
531
.......................................
Foreword
T
he invention of the bipolar junction transistor and the junction field-effect transistor by Bardeen, Brattain, and Shockley in 1956 foreshadowed the development of generations of smart phones and computers yet to come. The invention of the silicon integrated circuit (IC) by Jack Kilby of Texas Instruments in 1958 and 6 months later by Robert Noyce of Fairchild Semiconductor excited the development of generations of integrations. The proposal of doubling the number of transistors on an IC every 24 months by Gordon Moore in 1965 (also called Moore’s law) has been the most powerful driver for the development of the microelectronic industry in the past 44 years. This law emphasizes lithography scaling and integration (in two dimensions) of all functions on a single chip, through system-on-chip (SoC). Apart from SoC, integration of all these functions can be achieved through system-in-package (SiP) or, ultimately, three-dimensional IC integration, which can be called “more than Moore.” Based on siliconplatform technology, anything that involves the integration of electronics, photonics, mechanics, chemistry, heat, magnetics, biology, etc., for functionality and system performance when interacting with people and the environment is known as more than Moore. Microelectromechanical systems (MEMS) is a part of it. Yole Development forecasted the MEMS market to be $14 billion by 2012. The packaging cost of MEMS products in general is about 70 percent. Thus MEMS packaging could be a $10 billion market by 2012. Unlike electronics IC packaging, MEMS packaging is custombuilt and difficult due to the moving structural elements. For some MEMS devices, such as resonators, infrared bolometers, and gyroscopes, vacuum packaging is required. For most researchers and engineers, advanced MEMS packaging is the least understood of all. Thus, there is an urgent need to generate a comprehensive book on the current state of knowledge in the design, materials, process, manufacturing, and reliability of advanced MEMS packaging technology. Institute of Microelectronics (IME), Singapore, one of the research institutes of the Agency for Science, Technology and Research (A∗STAR), has been publishing MEMS papers extensively in a wide spectrum
xv
xvi
Foreword of journals, conference proceedings, symposia, and workshops. However, there is no single comprehensive compilation of information devoted to state-of-the-art advanced MEMS packaging. This book is written for everyone who can quickly learn about the basics and problem-solving methods, understand the trade-offs, and make system-level decisions. John Lau, Chengkuo Lee, C. S. Premachandran, and Yu Aibin of IME have taken the time and made the effort to complete this book on this timely topic of advanced MEMS packaging. This book will help focus the attention of practicing engineers and research scientists, as well as faculty and students, on the complex MEMS packaging challenges that must be overcome. I wish that this book will serve future generations of engineers, scientists, and students who will continue to advance the science and engineering of MEMS packaging. With their predecessors’ knowledge and their creativity, there is no doubt this wish will come true. Professor Dim-Lee Kwong Executive Director Institute of Microelectronics Singapore
Preface
T
he last decade witnessed an explosive growth in research and development efforts devoted to advanced microelectromechanical systems (MEMS) packaging as a direct result of higher requirements for package footprint, density, and performance and cost advantages over conventional MEMS packages. For the next decade, MEMS devices and packaging will penetrate into IT, telecommunications, automotive, life sciences, medical, and implantable applications. However, like many other new technologies, advanced MEMS packaging still has many critical issues that need to be addressed. In the development of advanced MEMS packaging, the following must be noted and understood: The infrastructure of MEMS devices and MEMS packaging is not well established; MEMS packaging expertise is not commonly available; MEMS packaging is unique and custom-built; MEMS general packaging platform technology is not available; hermetic sealing of the MEMS device is necessary; vacuum packaging is even required for some MEMS devices; vertical electrical feed-through with through-silicon vias (TSVs) is still too costly; bare ASIC die/wafers are not commonly available for three-dimensional (3D) integration; bare thin die/wafer handling is not easy; pick and place is more difficult; low-temperature bonding is not mature enough for high-volume production; rework is more difficult; micro solder bumping, assembly, and reliability are more critical; inspection is more difficult; MEMS assembly testability is not well established; dies shrink and expand; known-good-die; thermal management; wafer dicing; and device/chip cracking during bonding. In the past few years, some of these critical issues have been studied by experts in the field. Their results have been disclosed in diverse journals and in the proceedings of many conferences, symposia, and workshops whose primary emphases are electrical designs, materials science, manufacturing engineering, or electronic packaging and interconnection. Consequently, there is no single source of information devoted to the state of the art of advanced MEMS packaging technologies for, e.g., inertial, optical, RF, BioMEMS, and medical MEMS devices. This book aims to remedy this deficiency
xvii
xviii
Preface by presenting in one complete and concise volume a summary of the progress in this fascinating field that has occurred within the past few years. This book is written for everyone so that they can quickly learn the basics, grasp problem-solving methods, understand the tradeoffs, and make system-level decisions with advanced MEMS packaging technologies. This book is organized into five parts. Chapter 1, the first part, briefly discusses MEMS devices, commercial applications, and markets. MEMS packaging is also briefly mentioned, and some of the MEMS packaging patents from the United States, Japan, and the world since 2001 are provided. Chapter 2, the second part, briefly discusses the state of the art and future trends of advanced integrated-circuit (IC) electronics packaging. It is followed by advanced MEMS packaging, where 10 different designs of 3D MEMS packaging and their assembly processes are presented. There are two chapters in the third part, where some important enabling technologies for advanced MEMS packaging are presented. In Chapter 3, TSVs, stress sensors, wafer thinning and thin-wafer handling, low-temperature C2C, C2W, and W2W bonding, wafer dicing, and the reliability of RoHS-compliant MEMS packaging are discussed. Chapter 4 focuses on wafer-level packaging, where micromachining, wafer-level encapsulation, wafer-level chip capping, and a couple of case studies on wafer bonding based on low-temperature solder for MEMS packaging are presented. The fourth part has six chapters, and its focus is on the applications of advanced packaging on some MEMS devices. Chapter 5 presents an overview of microfabrication technology and major actuation mechanisms in enabling optical MEMS, followed by two well-studied optical MEMS devices in communications: optical switches and variable optical attenuators (VOAs). All aspects of MEMS design, manufacturability, packaging, and reliability are discussed. Chapter 6 presents the packaging and thermal reliability of the solder sealing ring of an RoHS-compliant 3D bubble-actuated photonic crossconnect switch. Emphasis is placed on determination of the thermal fatigue life of the lead-free solder sealing ring under shipping, storing, and handling conditions. Chapter 7 outlines the design, process, packaging, and testing of a bolometer vacuum package. The challenge of vacuum packaging and maintaining the temperature within ±0.1°C, packaging material and getter selections, and testing are presented. Chapter 8 presents the design, materials, process, and testing of bio-MEMS packaging. Emphasis is placed on the process developments of the microfluidics package and its application to extracting dengue virus from the samples. Chapter 9 presents the design, materials, process, and testing of MEMS packaging of a biosensor (micromirror) in an optical probe, which can take images from body tissues. Chapter 10 presents a wafer-level package with
Preface TSV interconnects and a wafer-level vacuum package with lateral electrical feed-through interconnects for accelerometer devices. For TSV interconnects, the die shear and hermeticity tests are used to characterize the package, and their results are discussed. For waferlevel vacuum packages, the C-V curves subjected to reliability tests and the Q-factor measurement of the vacuum inside the package are presented. The fifth part of this book covers radio frequency (RF) MEMS and packaging. Chapter 11 presents the design, fabrication, and characterization of RF MEMS switches. Emphasis is placed on mechanical and electrical design for performance, the micromachining and bulk micromachining processes, and maintaining an insertion loss of the MEMS switch that is lower than 0.5 dB up to 40 GHz and an isolation higher than 15 dB at 10 GHz. Chapter 12 presents different RF MEMS circuits, including tunable capacitors and tunable band-pass filters, which consist of different MEMS switches and can be tuned analogically or digitally. Usually the digital tuning approach has a larger tuning range and has more flexibility for constructing different tuning circuits. Chapter 13 presents the zero-level and first-level packaging of RF MEMS switches, which must be packaged in a nitrogen or dryair atmosphere (for high reliability) owing to hermeticity, temperature, and outgassing constraints. In zero-level packaging, capping of RF MEMS devices can be categorized as chip capping and thin-film capping. In first-level packaging, plastic packaging is the most common solution applicable for frequencies below several gigahertz, and ceramic packages exhibit the potential for good performance into the millimeter-wave region. For whom is this book intended? Undoubtedly, it will be of interest to three groups of specialists: (1) those who are active or intend to become active in research and development of MEMS devices and packaging, (2) those who have encountered practical MEMS packaging problems and wish to understand and learn more methods for solving such problems, and (3) those who have to choose a reliable, creative, high-performance, robust, and cost-effective packaging technique for their MEMS devices. This book also can be used as a text for undergraduate and graduate students who have the potential to become our future leaders, scientists, and engineers in the electronics, optoelectronics, and photonics industries. We hope that this book will serve as a valuable reference source for all those faced with the challenging problems created by the everincreasing interest in MEMS devices and packaging. We also hope that it will aid in stimulating further research and development on optical, electrical, thermal, and mechanical designs, materials, processes, manufacturing, testing, and reliability and more sound applications of advanced packaging technologies in MEMS products. The organizations that learn how to design advanced MEMS packaging in their interconnect systems have the potential to make
xix
xx
Preface major advances in the electronics industry and to gain great benefits in cost, performance, quality, size, and weight. It is our hope that the information presented in this book may assist in removing road blocks, avoiding unnecessary false starts, and accelerating design, materials, and process development of MEMS packaging. We are strongly against the notion that packaging is the bottleneck of advanced MEMS applications. Rather, we would like to consider this as a golden opportunity to make a major contribution to the MEMS industry by developing innovative, high-performance, cost-effective, and reliable packaging for MEMS products. It is an exciting time for advanced (especially 3D) MEMS packaging! John H. Lau Chengkuo Lee C. S. Premachandran Yu Aibin
Acknowledgments
D
evelopment and preparation of Advanced MEMS Packaging was facilitated by the efforts of a number of dedicated people. We would like to thank them all, with special mention to Michael Mulcahy of McGraw-Hill and Somya Rustagi of Glyph International for their unswerving support and advocacy. Our special thanks go to Taisuke Soda and Steve Chapman of McGraw-Hill, who made our dream of this book come true by effectively sponsoring the project, patiently listening to our excuses for delay, and solving many problems that arose during the book’s preparation. It has been a great pleasure and fruitful experience to work with all of them in transferring our messy manuscripts into a very attractive printed book. The material in this book clearly has been derived from many sources, including individuals, companies, and organizations, and we have attempted to acknowledge by citations, in the appropriate parts of the book, the assistance that we have been given. It would be quite impossible for us to express our thanks to everyone concerned for their cooperation in producing this book, but we would like to extend due gratitude. Also, we want to thank several professional societies and publishers for permitting us to reproduce some of their illustrations and information in this book, including the American Society of Mechanical Engineers (ASME) Conference Proceedings (e.g., International Intersociety Electronic Packaging Conference) and Transactions (e.g., Journal of Electronic Packaging), the Institute of Electrical and Electronic Engineers (IEEE) Conference Proceedings (e.g., Electronic Components & Technology Conference) and Transactions (e.g., Advanced Packaging, Components and Packaging Technologies, and Manufacturing Technology), the International Microelectronics and Packaging Society (IMAPS) Conference Proceedings (e.g., International Symposium on Microelectronics) and Transactions (e.g., International Journal of Microcircuits & Electronic Packaging), the IBM Journal of Research and Development, Electronic Packaging & Production, Advanced Packaging, Circuits Assembly, Surface Mount Technology, Connection Technology, Solid State Technology, Circuit World, Microelectronics International, and Soldering and Surface Mount Technology.
xxi
xxii
Acknowledgments John Lau would like to thank his former employers, the Institute of Microelectronics (IME), Agilent, and HP, for providing him excellent working environments that have nurtured him as a human being, fulfilled his need for job satisfaction, and enhanced his professional reputation. He also would like to thank Professor Dim-Lee Kwong for his trust, respect, and support of his work at IME, Agency for Science, Technology and Research (A∗STAR), Singapore. Furthermore, he would like to thank Dr. Lim Thiam Beng for helping to bring him into IME and all the members of the Microsystems, Modules, and Components Laboratory for their stimulating discussions, teamwork, and friendship. With respect to this book, Dr. Lau would like to single out the significant contributions of Zhang Xiaowu, Tang Gongyue, Cheryl Selvanayagam, Aditya Kumar, Yan Li Ling, Choi Won Kyoung, Kelvin Chen, Ahmad Kharyanto Bin Ratmin, Navas Khan, Chai Tai Chong, Yu Da Quan, N. Ranganathan, Ebin Liao, Li Hong Yu, Qing Xin Zhang, Seung Yoon, Feng Hanhua, Xie Ling, Ong Yue Ying, Wai Yin Hnin, Eva Wai, Damaruganath Pinjala, Vaidyanathan Kripesh, and Joanne Tan. Finally, he would like to thank his eminent colleagues (the enumeration of whom would not be practical here) at HKUST, IME, HP, and Agilent and throughout the electronics industry for their useful help, strong support, and stimulating discussions. Working and socializing with them has been a privilege and an adventure. He learned a lot about life and advanced packaging and interconnection technologies from them. Chengkuo Lee would like to thank his colleagues at Asia Pacific Microsystems, Inc., in Hsinchu, Taiwan, for their excellent work in MEMS packaging technology development. In particular, Mr. Ming Hung Tasi, Mr. Chia-Yu Wu, Mr. Chihchung Chen, Dr. Yen-Jyh Lai, Mr. Yu-Shen Lin, Mr. Shih-Yun Hung, Mr. Wen-Chih Chen, Dr. ShihChin Gong, and Professor Ruey-Shing Huang are specially acknowledged. Dr. Lee also appreciates his colleagues at the Institute of Microelectronics, A∗STAR, Singapore, for their research work in MEMS wafer-level packaging technology. To name a few, Dr. Daquan Yu, Dr. Li Ling Yan, Dr. Won Kyoung Choi, Dr. Johnny H. He, Dr. Qing Xin Zhang, Dr. Seung-Uk Yoon, and Dr. Hanhua Feng are appreciated most. Dr. Lee extends thanks to Mr. Riko I Made and Professor Chee Lip Gan from the School of Materials Science and Engineering, Nanyang Technological University, for their work in InAg solder bonding. He is further indebted to Professor J. Andrew Yeh at National Tsing Hua University, Hsinchu, Taiwan; Professor T. Suga, Professor H. Toshiyoshi, and Professor H. Fujita at the University of Tokyo, Tokyo, Japan; Dr. R. Maeda, Dr. T. Itoh, and Dr. T. Kobayashi of AIST, Tsukuba, Japan; Professor R. Sawada at Kyushu University, Fukuoka, Japan; Professor R. R. A. Syms at Imperial College, London, United Kingdom; and Professor Lih Y. Lin at the University of Washington, Seattle, Washington, for information on their research results and their continuous support. Dr. Lee also
Acknowledgments acknowledges Professor C.-C. Chen at the National Central University, Jhong-Li, Taiwan, and Professor John T. L. Thong, Professor W. K. Choi, Professor G. Pastorin, and Dr. Fu-Li Hsiao at the National University of Singapore for their continuous support and encouragement. C. S. Premachandran would like to acknowledge and thank his colleagues Ling Xie and Michelle Chew for their contribution on bioMEMS packaging; Dr. Pavel Neuzil, Chong Ser Choong, Navas Khan, Damaruganath Pinjala, Chai Tai Chong, and Dr. Zhang Xiao Wu for their contribution on optical MEMS—bolometer packaging; Dr. Janak Singh, Xu Yingshun, Kelvin Chen, Ahmad Khairyanto, Pamidighantam Ramana, Chuah Tong Kuan, and Jaya Krishnan Chandrappan for their contribution on biosensor packaging; and Dr. Mahadevan K. Iyer, Rangnathan Nagarajan, Choong Ser Chong, Mihai D. Rotaru, Dr. Chen Yu, and Dr. Vaidyanathan Kripesh for their contribution on accelerometer packaging. Finally, he would like to thank Dr. Lim Thiam Beng, who has inspired him in the MEMS packaging research area. Yu Aibin would like to thank all the authors cited in the reference lists for sharing their important and useful knowledge. He also would like to thank Professor AiQun Liu from Nanyang Technological University, Singapore, and Dr. Zhang Qingxin from the Institute of Microelectronics, Singapore, for invaluable support. Lastly, John Lau wants to thank his daughter Judy and his wife Teresa for their love, consideration, and patience by allowing him to work peacefully on this book. Their simple belief that he is making a small contribution to the electronics industry was a strong motivation for him. Knowing that Judy has earned her Ph.D. degree in physics from Princeton University and is working for Stanford University and that Teresa and he are in good health, he wants to thank God for his generous blessings. Chengkuo Lee shares the same feelings about his family. For a certain period of time, he slept only 4 hours a day on average while working on this book. Without the spiritual support of his family, he could never have struggled through those exhausting nights! C. S. Premachandran would like to thank his wife, Asha Venugopal, and their loving children, Karthik and Swetha, for their continuous support, love, and understanding while he worked on this book. Yu Aibin wishes to express his gratitude to his parents for all their support through the years; to his wife, Zhu Suli, for her understanding and loving support; and to his lovely daughter, Yu Wanxin, for her joyful time.
xxiii
This page intentionally left blank
CHAPTER
1
Introduction to MEMS 1.1
Introduction MEMS stand for microelectromechanical systems, which are the integration of mechanical elements such as sensors and actuators and electronics on a common silicon substrate through the use of microfabrication technology.1–41 The same basic technology and process steps such as the etching, patterning, doping, and connecting employed for making conventional electronic integrated circuits (ICs) such as complementary metal-oxide-semiconductors (CMOS) can be used to fabricate (micromachining) micromechanical elements by selectively etching away parts of a silicon wafer or adding new structural layers to form MEMS devices. However, there is a fundamental difference between MEMS and ICs devices—namely, MEMS devices must remain physically movable. MEMS devices use electronics to move their mechanical elements (parts)! MEMS are made up of elements between 1 and 100 μm (0.001 and 0.1 mm) in size, and MEMS devices generally range in size from 20 to 1000 μm.42 Nanoelectromechanical systems (NEMS) are similar to MEMS but much smaller, and they hold the promise of improving the ability to measure infinitesimal displacements and forces on the molecular scale but will not be discussed in this book. Micro-opto-electromechanical systems (MOEMS) are a special class of MEMS that use electronics to move mechanical parts that can sense and control light and manipulate optical signals. Their fabrication technology and process are similar to those of MEMS except that in addition to silicon materials, they also use, for example, gallium arsenide.
1
2 1.2
Chapter One
Commercial Applications of MEMS MEMS provide a combination of mechanical functions (e.g., sensing, moving, and heating) and electrical functions (e.g., switching and deciding). Some commercial applications42 of MEMS today are as follows: • Inkjet printers, which use piezoelectric or thermal bubble ejection to deposit ink on paper • Accelerometers in modern cars for a large number of purposes, including airbag deployment in collisions • Accelerometers in consumer electronic devices such as game controllers (Nintendo Wii), personal media players/cell phones (Apple iPhone), and a number of digital cameras (various Canon Digital IXUS models), as well as in PCs to park the hard-disk head when free fall is detected to prevent damage and data loss • MEMS gyroscopes used in modern cars and other applications to detect yaw (e.g., to deploy a roll-over bar or trigger dynamic stability control) • Silicon pressure sensors such as car tire-pressure sensors and disposable blood pressure sensors • Displays in projectors (e.g., the DMD chip) based on DLP technology, which has on its surface several hundred thousand micromirors • Optical switching technology such as that used for switching and aligning data communications • Bio-MEMS applications in medical and health related technologies from Lab-On-a-Chip to MicroTotalAnalysis (e.g., biosensors and chemosensors) • Interferometric modulator displays (IMOD) in consumer electronics (primarily displays for mobile devices), which are used to create interferometric modulation (i.e., reflective display technology as found in Mirasol displays)
1.3
MEMS Markets The MEMS market forecast by Yole Development calls for $10 billion by 2010 and $14 billion by 2012. [For 2008, Jean Christophe Eloy, CEO of Yole, expects the market to be $7.8 billion. This represents a combined annual growth rate (CAGR) of 14 percent for the 2007–2012 period. The 2007–2010 growth, however, will be quite modest (11 percent), but strong growth is expected after 2010.] The packaging cost of a MEMS product
Introduction to MEMS in general is between 60 and 80 percent. Thus MEMS packaging could be a $7 billion market by 2010 and $10 billion by 2012. The MEMS devices that make up the market forecast are, for example, inkjet (IJ) heads, pressure sensors, silicon microphones, accelerometers, gyroscopes, MOEMS devices, microbolometers, microdisplays, microfluidics, radiofrequency (RF) MEMS, microtips, microfuel cells, and emerging MEMS. These MEMS devices can be applied to the automotive, aeronautics, consumer, defense, industrial, medical, life science, and telecommunication industries. Their units and market values have been provided by Yole Development and are shown in Figs. 1-1 and 1-2, which also include the forecasts up to 2012. It can be seen that the value of MEMS production is expected to double in 2012 (from 2007) and that the total units of MEMS production are expected to quadruple in 2012 (from 2007). According to Jean Christophe Eloy, whose company tracks 150 MEMS applications, RF MEMS is expected to have the highest growth (50 percent) (Figs. 1-3 and 1-4), followed by microfluidic chips for drug delivery (42 percent), silicon microphones (32 percent), microfluidic chips for diagnostics (23 percent), microtips and microprobes (22 percent), and microbolometers (20 percent). Eloy also said that the most promising MEMS devices include accelerometers for humanmachine interfaces, with a CAGR exceeding 120 percent, followed by RF-MEMS devices for automatic test equipment (81 percent).
16,000.0 Defense
14,000.0
Aeronautics
Million, $ US
12,000.0
Industrial
10,000.0
Telecom
8,000.0
Life science
6,000.0
Medical 4,000.0 Automotive 2,000.0
Consumer
0.0 2006 Consumer Automotive Medical Lifescience Telecom Industrial Aeronautics Defense
2007
2008
2009
2010
2011
2012
2006
2007
2008
2009
2010
2011
2012
854.4 375.6 49.6 154.5 257.8 23.7 0.3 0.8
997.9 422.7 58.1 173.4 386.2 25.2 0.3 1.1
1,231.0 480.5 70.8 199.2 539.9 27.9 0.4 1.4
1,531.9 510.7 85.5 228.8 799.2 36.3 0.5 1.8
1,999.3 541.1 112.0 274.7 1,274.4 49.5 0.5 2.1
2,689.8 571.4 132.1 367.7 2,005.9 64.2 0.6 2.4
3,504.4 615.3 139.5 494.4 3,214.7 154.9 0.6 3.2
FIGURE 1-1 MEMS value market forecast for 2006–2012 ($ US millions).
3
Chapter One
Million, units
9,000.0 8,000.0
Defense
7,000.0
Aeronautics
6,000.0
Industrial
5,000.0
Telecom
4,000.0
Life science
3,000.0
Medical
2,000.0
Automotive
1,000.0 Consumer 0.0 2006 Consumer Automotive Medical Life science Telecom Industrial Aeronautics Defense
2007
2008
2009
2010
2011
2012
2006
2007
2008
2009
2010
2011
2012
2,825.2 1,277.7 336.0 432.6 380.4 853.9 30.0 258.1
2,919.4 1,362.2 381.3 494.6 556.3 912.0 37.8 343.2
3,322.3 1,421.8 422.8 573.4 650.2 991.4 45.4 415.3
3,639.7 1,464.7 457.7 664.3 791.4 1,107.2 52.6 489.3
4,129.2 1,464.0 495.2 788.6 1,002.5 1,244.9 59.8 558.9
4,608.6 1,485.9 535.7 1,254.6 1,325.2 1,439.8 66.0 628.9
5,415.3 1,572.4 560.1 1,645.6 1,827.7 1,945.3 78.5 824.8
FIGURE 1-2 MEMS volume market forecast for 2006–2012 (millions of units).
1,600.0 1,400.0
Million, $ US
4
1,200.0 1,000.0 800.0
RF-MEMS for consumer RF-MEMS for defense RF-MEMS for aeronautics RF-MEMS for industrial RF-MEMS for telecom
600.0 400.0 200.0 0.0 2006 2007 2008 2009 2010 2011 2012
RF-MEMS for telecom RF-MEMS for industrial RF-MEMS for aeronautics RF-MEMS for defense RF-MEMS for consumer
2006
2007
2008
2009
2010
2011
2012
179.0
321.1
385.5
467.9
632.4
888.2
1,284.9
1.0
4.5
9.4
17.6
36.1
56.9
95.8
0.0
0.0
0.0
0.0
0.1
0.1
0.2
0.2
0.8
2.1
4.3
9.0
14.1
22.9
0.0
0.5
2.0
5.0
10.0
20.0
25.0
FIGURE 1-3 RF-MEMS value market forecast for 2006–2012 ($US millions).
Introduction to MEMS 2,500.0
Million, units
2,000.0 1,500.0
RF-MEMS for consumer RF-MEMS for defense RF-MEMS for aeronautics RF-MEMS for industrial RF-MEMS for telecom
1,000.0 500.0 0.0 2006 2007 2008 2009 2010 2011 2012
RF-MEMS for telecom RF-MEMS for industrial RF-MEMS for aeronautics RF-MEMS for defense RF-MEMS for consumer
2006
2007
2008
2009
2010
2011
2012
3.0
5.0
8.3
96.4
371.0
894.7
1,826.2
0.0
0.2
0.4
0.9
2.6
5.3
11.7
0.0
0.0
0.0
0.0
0.0
0.0
0.0
0.0
0.0
0.0
0.0
0.0
0.1
0.1
0.0
5.0
20.0
50.0
100.0
200.0
250.0
FIGURE 1-4 RF-MEMS volume market forecast for 2006–2012 (millions of units).
1.4 Top 30 MEMS Suppliers The top 30 MEMS suppliers ranked by Yole Development 43 are Hewlett-Packard (HP), Texas Instruments (TI), Robert Bosch, Lexmark, Seiko Epson, STMicroelectronics, Freescale Semiconductor, Canon, Analog Devices, Systron Donner, Denso, Avago Technologies, GE Sensing, Honeywell, Infineon Technology, Delphi, Olivettii-Jet, Boehringer Ingelheim Microparts, VTI Technologies, Panasonic, Formfactor, Knowles Electronics, Murata, Continental Automotive, Measurement Specialties, Inc., Flir Systems, Ulis, Omron, Silicon Sensing Systems, and Colibrys. These 30 companies’ global sales totaled approximately $6 billion in 2007, representing approximately 80 percent of the global MEMS market. HP is the largest supplier, mainly supplying inkjet printheads, followed by TI, which mainly provides the digital light processor. For more information about these companies and many others, please see ref. 43.
1.5
Introduction to MEMS Packaging The MEMS device is not an isolated island. It must communicate with other integrated circuit (IC) chips in a circuit through an input/ output (I/O) system of interconnects. Furthermore, the MEMS device needs to be powered up, and its embedded circuitry and elements are
5
6
Chapter One delicate, requiring the package to both carry and protect the device. Consequently, the major functions of MEMS packaging are (1) to provide a path for the electrical current that powers the circuit and moves the moving elements, (2) to distribute the signals onto and off the MEMS device, (3) to remove the heat generated by the circuit, and (4) to support and protect the MEMS device from hostile environments. Unlike electronics IC packaging,44–56 MEMS packaging is not trivial, is expensive (60 to 80 percent of the product total cost), and is custom-built. Electronics IC packaging is a well-developed technology (e.g., wire bonding, tape automated bonding, and the flip chip). However, MEMS packaging is a specially designed packaging process that is difficult owing to moving structural elements, and it is the most expensive process in micromachining. Unlike electronics IC packaging,44–56 MEMS packaging needs a cap. In order for the moving elements of a MEMS device to move effectively (e.g., with minimum damping and stiction) in a well-controlled atmosphere, hermetic sealing of the MEMS device in a cap is necessary. For some MEMS devices (e.g., resonators, infrared bolometers, and gyroscopes), vacuum packaging is even required. Usually, the cap is processed at the wafer level, and thus MEMS packaging is truly a waferlevel packaging. The design, materials, process, testing, and reliability of MEMS wafer-level packaging will be presented, discussed, and examined throughout this book.
1.6
MEMS Packaging Patents since 2001 In the past few years, many patents have been granted for MEMS packaging. In this section, some of the patents (since 2001) from the United States, Japan, and the world have been selected and listed for convenient practice.
1.6.1
U.S. MEMS Packaging Patents
Some of the U.S. MEMS packaging patents selected from the U.S. Patent and Trademark Office (USPTO) since 2001 are as follows: Patent No. 7,508,063
7,491,567
7,479,516
Owner(s)/Title/Date Duboc, Robert M. (Menlo Park, CA), Tarn, Terry (San Diego, CA), “Low cost hermetically sealed package,” March 24, 2009. D’Camp, Jon B. (Savage, MN), Curtis, Harlan L. (Champlin, MN), “MEMS device packaging methods,” February 17, 2009. Chen, Jian (Richardson, TX), Rajagopal, Ramasubramaniam (Richardson, TX), “Nanocomposites and methods thereto,” January 20, 2009.
Introduction to MEMS 7,465,600
7,463,404
7,456,497
7,452,800
7,449,784
7,449,358
7,449,356
7,443,563
7,436,054
7,425,749
Michael, Don (Monmoth, OR), Rossman, Mari J. (Corvallis, OR), Bower, Bradley (Junction City, OR), Haluzak, Charles Craig (Corvallis, OR), Stemer, John R. (Albany, OR), Qi, Quan (Corvallis, OR), Kane, John (Corvallis, OR), “Package for a micro-electro-mechanical device,” December 16, 2008. Chen, Dongmin (Saratoga, CA), Xiong, Fulin (San Jose, CA), “Method of using a preferentially deposited lubricant to prevent anti-stiction in micromechanical systems,” December 9, 2008. Higashi, Mitsutoshi (Nagano, JP), “Electronic devices and its production methods,” November 25, 2008. Sosnowchik, Brian D. (Walnut Creek, CA), Lin, Liwei (Castro Valley, CA), Pisano, Albert P. (Danville, CA), “Bonding a non-metal body to a metal surface using inductive heating,” November 18, 2008. Sherrer, David W. (Radford, VA), Rasnake, Larry J. (Blacksburg, VA), Fisher, John J. (Blacksburg, VA), “Device package and methods for the fabrication and testing thereof,” November 11, 2008. Patel, Satyadev R. (Sunnyvale, CA), Huibers, Andrew G. (Palo Alto, CA), Chiang, Steve S. (Saratoga, CA), “Methods for depositing, releasing and packaging micro-electromechanical devices on wafer substrates,” November 11, 2008. Weigold, Jason W. (Somerville, MA), “Process of forming a microphone using support member,” November 11, 2008. Palmateer, Lauren (San Francisco, CA), Gally, Brian J. (Los Gatos, CA), Cummings, William J. (Millbrae, CA), Kothari, Manish (Cupertino, CA), Chui, Clarence (San Jose, CA), “Packaging for an interferometric modulator,” October 28, 2008. Zhe, Wang (Singapore, SG), “MEMS microphone with a stacked PCB package and method of producing the same,” October 14, 2008. Hartzell, John Walter (Camas, WA), Zhan, Changqing (Vancouver, WA), Wolfson, Michael Barrett (Somerville, MA), “MEMS pixel sensor,” September 16, 2008.
7
8
Chapter One 7,424,198
7,422,962
7,416,938
7,415,870
7,414,310
7,408,250
7,405,860
7,405,466
7,405,100
7,402,878
Palmateer, Lauren (San Francisco, CA), Cummings, William J. (San Francisco, CA), Gally, Brian (San Rafael, CA), Miles, Mark (San Francisco, CA), Sampsell, Jeffrey B. (San Jose, CA), Chui, Clarence (San Mateo, CA), Kothari, Manish (Cupertino, CA), “Method and device for packaging a substrate,” September 9, 2008. Chen, Chien-Hua (Corvallis, OR), Chen, Zhizhang (Corvallis, OR), Geissler, Steven R (Albany, OR), “Method of singulating electronic devices,” September 9, 2008. Seh, Huankiat (Phoenix, AZ), Min, Yongki (Phoenix, AZ), “Inkjet patterning for thin-film capacitor fabrication, thin-film capacitors fabricated thereby, and systems containing same,” August 26, 2008. Mancosu, Federico (Milan, IT), Brusarosco, Massimo (Cesano Boscone, IT), Fioravanti, Anna Paola (Monza, IT), Romeo, Fabio (Monza, IT), “Movable unit and system for sensing at least one characteristic parameter of a tyre,” August 26, 2008. Do, Byung Tai (Singapore, SG), Yang, Sung Uk (Singapore, SG), “Waferscale package system,” August 19, 2008. Doan, Jonathan (Mountain View, CA), Tarn, Terry (San Diego, CA), “Micromirror array device with compliant adhesive, August 5, 2008. Huibers, Andrew G. (Mountain View, CA), Patel, Satyadev R. (Elk Grove, CA), “Spatial light modulators with light blocking/absorbing areas,” July 29, 2008. Wei, Jun (Singapore, SG), Wong, Stephen Chee Khuen (Singapore, SG), Wu, Yongling (Singapore, SG), Ng, Fern Lan (Singapore, SG), “Method of fabricating microelectromechanical system structures,” July 29, 2008. Mostafazadeh, Shahram (San Jose, CA), Smith, Joseph O. (Morgan Hill, CA), “Packaging of a semiconductor device with a non-opaque cover,” July 29, 2008. Tarn, Terry (San Diego, CA), “Packaging method for microstructure and semiconductor devices,” July 22, 2008.
Introduction to MEMS 7,393,758
7,393,712
7,381,629
7,381,583
7,378,734
7,373,026
7,368,808
7,368,311
7,361,581
7,358,106
Sridhar, Uppili (Dallas, TX), Zou, Quanbo (Plano, TX), “Wafer level packaging process,” July 1, 2008. Smith, Mark A. (Corvallis, OR), Boucher, William R (Corvallis, OR), Haluzak, Charles C (Corvallis, OR), “Fluidic MEMS device,” July 1, 2008. Sankarapillai, Chirayarikathuveedu Premachandran (Singapore, SG), Nagarajan, Ranganathan (Singapore, SG), Soundarapandian, Mohanraj (Singapore, SG), “Method of forming through-wafer interconnects for vertical wafer level packaging,” June 3, 2008. Ebel, John L. (Beavercreek, OH), Cortez, Rebecca (Xenia, OH), Strawser, Richard E. (Greenville, OH), Leedy, Kevin D. (Centerville, OH), “MEMS RF switch integrated process,” June 3, 2008. Yabuki, Richard (Garden Grove, CA), Tea, Nim (Orange, CA), “Stacked contact bump,” May 27, 2008. Chui, Clarence (San Mateo, CA), “MEMS device fabricated on a pre-patterned substrate,” May 13, 2008. Heck, John (Palo Alto, CA), Hayden, III, Joseph S. (Sunnyvale, CA), Greathouse, Steve W. (Chandler, AZ), Wong, Daniel M. (Fremont, CA), “MEMS packaging using a non-silicon substrate for encapsulation and interconnection,” May 6, 2008. Tilmans, Hendrikus (Maastricht, NL), Beyne, Eric (Leuven, BE), Jansen, Henri (Leuven, BE), De Raedt, Walter (Edegem, BE), “Method and system for fabrication of integrated tunable/ switchable passive microwave and millimeter wave modules,” May 6, 2008. Adkisson, James W. (Jericho, VT), Gambino, Jeffrey P. (Westford, VT), Jaffe, Mark D. (Shelburne, VT), Rassel, Richard J. (Colchester, VT), Sprogis, Edmund J. (Underhill, VT), “High surface area aluminum bond pad for through-wafer connections to an electronic package,” April 22, 2008. Potter, Curtis Nathan (Austin, TX), “Hermetic MEMS package and method of manufacture,” April 15, 2008.
9
10
Chapter One 7,357,017
7,324,716
7,314,777
7,309,902
7,307,775
7,302,829
7,297,573
7,288,464
7,286,278
Felton, Lawrence E. (Hopkinton, MA), Harney, Kieran P. (Andover, MA), Roberts, Carl M. (Topsfield, MA), “Wafer level capped sensor,” April 15, 2008. Epitaux, Marc (Sunnyvale, CA), “Silicon packaging for opto-electronic modules,” January 29, 2008. D’Camp, Jon B. (Savage, MN), Curtis, Harlan L. (Champlin, MN), Dunaway, Lori A. (New Hope, MN), Glenn, Max C. (Chanhassen, MN), “Chip packaging systems and methods,” January 1, 2008. Reboa, Paul F. (Corvallis, OR), “Microelectronic device with anti-stiction coating,” December 18, 2007. Patel, Satayadev R. (Sunnyvale, CA), Huibers, Andrew G. (Palo Alto, CA), Chiang, Steve (Saratoga, CA), Duboc, Robert M. (Menlo Park, CA), Grobelny, Thomas J. (Snohomish, WA), Chen, Hung Nan (Kaohsiung, TW), Dehlinger, Dietrich (Sebastopol, CA), Richards, Peter W. (Palo Alto, CA), Shi, Hongqin (San Jose, CA), Sun, Anthony (San Jose, CA), “Methods for depositing, releasing and packaging microelectromechanical devices on wafer substrates,” December 11, 2007. Zribi, Anis (Rexford, NY), “Contactless humidity/chemical vapor sensor device and associated method of fabrication,” December 4, 2007. D’Camp, Jon B. (Savage, MN), Curtis, Harlan L. (Champlin, MN), Dunaway, Lori A. (New Hope, MN), Glenn, Max C. (Chanhassen, MN), “Methods and apparatus for particle reduction in MEMS devices,” November 20, 2007. Haluzak, Charles C. (Corvallis, OR), Pollard, Jeffrey R. (Corvallis, OR), “MEMS packaging structure and methods,” October 30, 2007. Patel, Satyadev R. (Sunnyvale, CA), Huibers, Andrew G. (Palo Alto, CA), Chiang, Steve S. (Saratoga, CA), “Methods for depositing, releasing and packaging micro-electromechanical devices on wafer substrates,” October 23, 2007.
Introduction to MEMS 7,282,329
7,276,789
7,276,398
7,275,424
7,262,622 7,259,449
7,243,533
7,238,999
7,238,546
7,233,048
7,218,742
7,217,588
7,203,394
Manalis, Scott (Cambridge, MA), Burg, Thomas (Cambridge, MA), “Suspended microchannel detectors,” October 16, 2007. Cohn, Michael B. (Berkeley, CA), Kung, Joseph T. (Santa Clara, CA), “Microelectromechanical systems using thermocompression bonding,” October 2, 2007. Michael, Don (Monmoth, OR), Rossman, Mari J. (Corvallis, OR), “System and method for hermetically sealing a package,” October 2, 2007. Felton, Lawrence E. (Hopkinton, MA), Harncy, Kieran P. (Andover, MA), Roberts, Carl M. (Topsfield, MA), “Wafer level capped sensor,” October 2, 2007. Zhao, Yang (Andover, MA), “Wafer-level package for integrated circuits,” August 28, 2007. Floyd, Philip D. (Redwood City, CA), “Method and system for sealing a substrate,” August 21, 2007. Mancosu, Federico (Milan, IT), Romeo, Fabio (Monza, IT), Brusarosco, Massimo (Cesano Boscone, IT), Fioravanti, Anna Paolo (Monza, IT), “Movable unit and system for sensing at least one characteristic parameter of a tyre,” July 17, 2007. LaFond, Peter H. (Redmond, WA), Yu, Lianzhong (Redmond, WA), “High performance MEMS packaging architecture,” July 3, 2007. Stark, David H. (Evergreen, CO), “Hermetically sealed micro-device package with window,” July 3, 2007. Rybnicek, Kimon (Santa Barbara, CA), “MEMS device trench plating process and apparatus for through hole vias,” June 19, 2007. Kay, Kelly Q. (Chicago, IL), Gilbert, Mark W. (Park Ridge, IL), “Condenser microphone assembly,” May 15, 2007. Hartzell, John W. (Camas, WA), Walton, Harry Garth (Beckley, GB), Brownlow, Michael James (Drayton, GB), “Integrated MEMS packaging,” May 15, 2007. Wiegele, Thomas (Apple Valley, MN), Apanius, Christopher (Moreland Hills, OH), Goldman, Kenneth G. (Olmsted Township, OH), Guo,
11
12
Chapter One
7,202,553
7,202,552
7,198,982
7,183,176
7,176,106
7,166,488
7,164,199
7,160,637
7,153,759
Shuwen (Lakeville, MN), St. Clair, Loren E. (Apple Valley, MN), O’Meara, Timothy R. (Burnsville, MN), Pohl, James J. (Apple Valley, MN), “Micro mirror arrays and microstructures with solderable connection sites,” April 10, 2007. Snyder, Tanya Jegeris (Edina, MN), Yi, Robert H. (Palo Alto, CA), Wilson, Robert Edward (Palo Alto, CA), “Wafer bonding using reactive foils for massively parallel micro-electromechanical systems packaging,” April 10, 2007. Zhe, Wang (Singapore, SG), Yubo, Miao (Singapore, SG), “MEMS package using flexible substrates, and method thereof,” April 10, 2007. Patel, Satyadev R. (Sunnyvale, CA), Huibers, Andrew G. (Palo Alto, CA), Chiang, Steve S. (Saratoga, CA), “Methods for depositing, releasing and packaging micro-electromechanical devices on wafer substrates,” April 3, 2007. Sankarapillai, Chirayarikathuveedu Premachandran (Singapore, SG), Nagarajan, Ranganathan (Singapore, SG), Soundarapandian, Mohanraj (Singapore, SG), “Method of forming through-wafer interconnects for vertical wafer level packaging,” April 3, 2007. Snyder, Tanya Jegeris (Edina, MN), Yi, Robert H. (Palo Alto, CA), Wilson, Robert Edward (Palo Alto, CA), “Wafer bonding using reactive foils for massively parallel micro-electromechanical systems packaging,” February 13, 2007. MacDonald, Noel C. (Santa Barbara, CA), Aimi, Marco F. (Goleta, CA), “Metal MEMS devices and methods of making same,” January 23, 2007. Tarn, Terry (San Diego, CA), “Device packages with low stress assembly process,” January 16, 2007. Chiao, Mu (Beaverton, OR), Lin, Liwei (Castro Valley, CA), Lam, Kien-Bang (Albany, CA), “Implantable, miniaturized microbial fuel cell,” January 9, 2007. Wei, Jun (Singapore, SG), Wong, Stephen Chee Khuen (Singapore, SG), Wu, Yongling (Singapore, SG), Ng, Fern Lan (Singapore, SG), “Method of fabricating microelectromechanical system structures,” December 26, 2006.
Introduction to MEMS 7,145,213
7,132,721
7,129,163
7,115,182
7,112,525
7,112,463
7,101,789
7,094,967
7,084,073
7,071,594
Ebel, John L. (Beavercreek, OH), Cortez, Rebecca (Xenia, OH), Strawser, Richard E. (Greenville, OH), Leedy, Kevin D. (Centerville, OH), “MEMS RF switch integrated process,” December 5, 2006. Platt, William P. (Columbia Heights, MN), Ford, Carol M. (Columbia Heights, MN), “Bonding for a micro-electro-mechanical system (MEMS) and MEMS based devices,” November 7, 2006. Sherrer, David W. (Radford, VA), Rasnake, Larry J. (Blacksburg, VA), Fisher, John J. (Blacksburg, VA), “Device package and method for the fabrication and testing thereof,” October 31, 2006. Wei, Jun (Singapore, SG), Wong, Stephen Chee Khuen (Singapore, SG), Nai, Sharon Mui Ling (Singapore, SG), “Anodic bonding process for ceramics,” October 3, 2006. Bhansali, Shekhar (Tampa, FL), Aravamudhan, Shyam (Tampa, FL), Luongo, Kevin (St. Petersburg, FL), Kedia, Sunny (Tampa, FL), “Method for the assembly of nanowire interconnects,” September 26, 2006. Horning, Robert (Savage, MN), Ohnstein, Thomas (Roseville, MN), Youngner, Daniel (Maple Grove, MN), “Method for making devices using ink jet printing,” September 26, 2006. Subramanian, Kanakasabapathi (Clifton Park, NY), Fortin, Jeffrey Bernard (Niskayuna, NY), Tian, Wei-Cheng (Clifton Park, NY), “Method of wet etching vias and articles formed thereby,” September 5, 2006. Evans, Cliff (Newtown, CT), Dalton, Mark William (Danbury, CT), “Electrical feedthru,” August 22, 2006. Lee, Moon-chul (Sungnam, KR), Choi, Hyung (Sungnam, KR), Jung, Kyu-dong (Suwon, KR), Jang, Mi (Suwon, KR), Hong, Seog-woo (Busan, KR), Chung, Seok-whan (Suwon, KR), Jun, Chan-bong (Seoul, KR), Kang, Seok-jin (Suwon, KR), “Method of forming a via hole through a glass wafer,” August 1, 2006. Yan, Jun (Cincinnati, OH), Casasanta, III, Vincenzo (Woodinville, WA), Luanava, Selso H. (Woodinville, WA), Urey, Hakan (Istanbul, TR),
13
14
Chapter One
7,030,432
7,029,829
7,011,793
7,008,193
7,004,015
7,002,436
7,002,241
7,002,215
6,995,040
DeWitt, IV, Frank A. (Bloomfield, NY), Tegreene, Clarence T. (Bellevue, WA), Wiklof, Christopher A. (Everett, WA), “MEMS scanner with dual magnetic and capacitive drive,” July 4, 2006. Ma, Qing (San Jose, CA), “Method of fabricating an integrated circuit that seals a MEMS device within a cavity,” April 18, 2006. Stark, Brian H. (Ann Arbor, MI), Najafi, Khalil (Ann Arbor, MI), “Low temperature method for forming a microcavity on a substrate and article having same,” April 18, 2006. Zhou, Peng (Newtown, PA), Young, Lincoln (Ithaca, NY), “Reconfigurable modular microfluidic system and method of fabrication,” March 14, 2006. Najafi, Khalil (Ann Arbor, MI), Kim, Hanseup S. (Ann Arbor, MI), Bernal, Luis P. (Ann Arbor, MI), Astle, Aaron A. (Ann Arbor, MI), Washabaugh, Peter D. (Ann Arbor, MI), “Micropump assembly for a microgas chromatograph and the like,” March 7, 2006. Chang-Chien, Patty P. L. (Hermosa Beach, CA), Wise, Kensall D. (Ann Arbor, MI), “Method and system for locally sealing a vacuum microcavity, methods and systems for monitoring and controlling pressure and method and system for trimming resonant frequency of a microstructure therein,” February 28, 2006. Ma, Qing (San Jose, CA), Cheng, Peng (Campbell, CA), Rao, Valluri (Saratoga, CA), “Vacuum-cavity MEMS resonator,” February 21, 2006. Mostafazadeh, Shahram (San Jose, CA), Smith, Joseph O. (Morgan Hill, CA), “Packaging of semiconductor device with a non-opaque cover,” February 21, 2006. Miller, David (Louisville, CO), “Floating entrance guard for preventing electrical short circuits,” February 21, 2006. Patel, Satyadev R. (Sunnyvale, CA), Huibers, Andrew G. (Palo Alto, CA), Chiang, Steve S. (Saratoga, CA), “Methods for depositing, releasing and packaging micro-electromechanical devices on wafer substrates,” February 7, 2006.
Introduction to MEMS 6,995,034
6,987,304
6,987,258
6,984,866
6,982,491
6,972,955
6,969,635
6,965,721
6,962,834
6,958,846
Patel, Satyadev R. (Sunnyvale, CA), Huibers, Andrew G. (Palo Alto, CA), Chiang, Steve S. (Saratoga, CA), “Methods for depositing, releasing and packaging micro-electromechanical devices on wafer substrates,” February 7, 2006. D’Camp, Jon B. (Savage, MN), Curtis, Harlan L. (Champlin, MN), Dunaway, Lori A. (New Hope, MN), Glenn, Max C. (Chanhassen, MN), “Methods and apparatus for particle reduction in MEMS devices,” January 17, 2006. Mates, John W. (Portland, OR), “Integrated circuit-based compound eye image sensor using a light pipe bundle,” January 17, 2006. Mostafazadeh, Shahram (San Jose, CA), Smith, Joseph O. (Morgan Hill, CA), Penry, Matthew D. (Morgan Hill, CA), “Flip chip optical semiconductor on a PCB,” January 10, 2006. Fan, Chun Ho (Sham Tseng, HK), Labeeb, Sadak Thamby (Tsuen Wan, HK), Chow, Lap Keung (Kowloon, HK), “Sensor semiconductor package and method of manufacturing the same,” January 3, 2006. Pleskach, Michael David (Orlando, FL), Koeneman, Paul Bryant (Palm Bay, FL), Smith, Brian Ronald (Pittsburgh, PA), Newton, Charles Michael (Palm Bay, FL), Gamlen, Carol Ann (Melbourne, FL), “Electro-fluidic device and interconnect and related methods,” December 6, 2005. Patel, Satyadev R. (Sunnyvale, CA), Huibers, Andrew G. (Palo Alto, CA), Chiang, Steven S. (Saratoga, CA), “Methods for depositing, releasing and packaging micro-electromechanical devices on wafer substrates,” November 29, 2005. Tullis, Barclay J. (Palo Alto, CA), Prince, John H. (Los Altos, CA), “Integrated manufacture of sidepolished fiber optics,” November 15, 2005. Stark, David H. (Evergreen, CO), “Wafer-level hermetic micro-device packages,” November 8, 2005. Huibers, Andrew G. (Mountain View, CA), Richards, Peter W. (Palo Alto, CA), “Spatial light modulators with light absorbing areas,” October 25, 2005.
15
16
Chapter One 6,956,283
6,953,985
6,952,301
6,949,398
6,936,918
6,936,494
6,924,974
6,917,099
6,906,847
6,902,656
Peterson, Kenneth A. (Albuquerque, NM), “Encapsulants for protecting MEMS devices during post-packaging release etch,” October 18, 2005. Lin, Jong-Kai (Chandler, AZ), Lytle, William H. (Chandler, AZ), Fay, Owen (Gilbert, AZ), Markgraf, Steven (Chandler, AZ), Hughes, Henry G. (Scottsdale, AZ), Amrine, Craig (Tempe, AZ), De Silva, Ananda P. (Chandler, AZ), “Wafer level MEMS packaging,” October 11, 2005. Huibers, Andrew G. (Palo Alto, CA), “Spatial light modulators with light blocking and absorbing areas,” October 4, 2005. Lytle, William H. (Chandler, AZ), Fay, Owen (Gilbert, AZ), Markgraf, Steven (Plymouth, MN), Springer, Stephen B. (Mesa, AZ), “Low cost fabrication and assembly of lid for semiconductor devices,” September 27, 2005. Harney, Kieran P. (Andover, MA), Felton, Lawrence E. (Hopkinton, MA), Nunan, Thomas Kieran (Carlisle, MA), Alie, Susan A. (Stoneham, MA), Wachtmann, Bruce (Concord, MA), “MEMS device with conductive path through substrate,” August 30, 2005. Cheung, Kin P. (Hoboken, NJ), “Processes for hermetically packaging wafer level microscopic structures,” August 30, 2005. Stark, David H. (Evergreen, CO), “Hermetically sealed micro-device package using cold-gas dynamic spray material deposition,” August 2, 2005. Hellekson, Ronald A. (Eugene, OR), Chen, Chien-Hua (Corvallis, OR), Boucher, William R (Corvallis, OR), Smith, Joshua W. (Corvallis, OR), Craig, David M (Albany, OR), Watts, Gary J. (Albany, OR), “Die carrier with fluid chamber,” July 12, 2005. Huibers, Andrew G. (Mountain View, CA), Patel, Satyadev R. (Elk Grove, CA), “Spatial light modulators with light blocking/absorbing areas,” June 14, 2005. Ouellet, Luc (Granby, CA), Antaki, Robert (St-Luc, CA), Tremblay, Yves (Brigham, CA), “Fabrication of microstructures with vacuumsealed cavity,” June 7, 2005.
Introduction to MEMS 6,900,072
6,894,383
6,876,056
6,858,466
6,853,067
6,846,725
6,844,959
6,844,623
6,838,047
6,835,594
Patel, Satyadev R. (Elk Grove, CA), Huibers, Andrew G. (Mountain View, CA), “Method for making a micromechanical device by using a sacrificial substrate,” May 31, 2005. Bar-Sadeh, Eyal (Jerusalem, IL), Talalyevsky, Alexander (Jerusalem, IL), Ginsburg, Eyal (Tel Aviv, IL), “Reduced substrate micro-electromechanical systems (MEMS) device and system for producing the same,” May 17, 2005. Tilmans, Hendrikus (Maastricht, NL), Beyne, Eric (Leuven, BE), Jansen, Henri (Leuven, BE), De Raedt, Walter (Edegem, BE), “Method and system for fabrication of integrated tunable/ switchable passive microwave and millimeter wave modules,” April 5, 2005. Bower, Bradley (Junction City, OR), Qi, Quan (Corvallis, OR), Sand, Kirby (Corvallis, OR), “System and a method for fluid filling wafer level packages,” February 22, 2005. Cohn, Michael B. (Berkeley, CA), Kung, Joseph T. (Santa Clara, CA), “Microelectromechanical systems using thermocompression bonding,” February 8, 2005. Nagarajan, Ranganathan (Singapore, SG), Premachandran, Chirayarikathuveedu Sankarapillai (Singapore, SG), Chen, Yu (Singapore, SG), Kripesh, Vaidyanathan (Singapore, SG), “Wafer-level package for microelectro-mechanical systems,” January 25, 2005. Huibers, Andrew G. (Mountain View, CA), Patel, Satyadev R. (Elk Grove, CA), Duboc, Jr., Robert M. (Menlo Park, CA), “Spatial light modulators with light absorbing areas,” January 18, 2005. Peterson, Kenneth A. (Albuquerque, NM), Conley, William R. (Tijeras, NM), “Temporary coatings for protection of microelectronic devices during packaging,” January 18, 2005. Billiet, Romain Louis (Penang, MY), Nguyen, Hanh Thi (Penang, MY), “MEMS and MEMS components from silicon kerf,” January 4, 2005. Shong, Ci-moo (Sungnam-si, KR), Kang, Seok-jin (Suwon-si, KR), Chung, Seok-whan (Suwon-si, KR), Lee, Moon-chul (Sungnam-si, KR), Jung, Kyu-dong (Suwon-si, KR), Kim, Jong-seok (Gyeonggi-do, KR), Jun, Chan-bong (Seoul, KR),
17
18
Chapter One
6,834,154
6,825,744
6,809,412
6,808,955
6,808,954
6,798,954
6,793,829
6,788,840
6,780,672
6,775,068
6,773,962
Hong, Seog-woo (Busan, KR), Kang, Jung-ho (Suwon-si, KR), “Metal wiring method for an undercut,” December 28, 2004. Carpenter, Barry S. (Oakdale, MN), “Tooling fixture for packaged optical micro-mechanical devices,” December 21, 2004. Harney, Kieran Patrick (Andover, MA), “Active alignment as an integral part of optical package design,” November 30, 2004. Tourino, Cory G. (Georgetown, TX), Rice, Janet L. (Austin, TX), Flynn, Gregory (Austin, TX), “Packaging of MEMS devices using a thermoplastic,” October 26, 2004. Ma, Qing (San Jose, CA), “Method of fabricating an integrated circuit that seals a MEMS device within a cavity,” October 26, 2004. Ma, Qing (San Jose, CA), Cheng, Peng (Campbell, CA), Rao, Valluri (Saratoga, CA), “Vacuum-cavity MEMS resonator,” October 26, 2004. Carpenter, Barry S. (Oakdale, MN), Hagen, Kathy L. (Stillwater, MN), Smith, Robert G. (Vadnais Heights, MN), “Packaged optical micro-mechanical device,” September 28, 2004. Platt, William P. (Columbia Heights, MN), Ford, Carol M. (Columbia Heights, MN), “Bonding for a micro-electro-mechanical system (MEMS) and MEMS based devices,” September 21, 2004. Stewart, Robert E. (Woodland Hills, CA), Cherbettchian, Agop H. (Santa Monica, CA), Fersht, Samuel (Studio City, CA), Hall, David B. (La Crescenta, CA), “Bi-stable micro-actuator and optical switch,” September 7, 2004. Steele, Daniel W. (Clay, NY), Chovan, Joseph L. (North Syracuse, NY), “Micro eletro-mechanical component and system architecture,” August 24, 2004. Lomas, Stuart John (Edmonton, CA), McLaughlin, Dean Edward (Baltimore, MD), “Integrated optical channel,” August 10, 2004. Saia, Richard Joseph (Niskayuna, NY), Durocher, Kevin Matthew (Waterford, NY), Kapusta, Christopher James (Duanesburg, NY),
Introduction to MEMS
6,771,859
6,767,764
6,760,500 6,759,590
6,723,379
6,716,767
6,696,645
6,696,343
6,661,069
Nielsen, Matthew Christian (Schenectady, NY), “Microelectromechanical system device packaging method,” August 10, 2004. Carpenter, Barry S. (Oakdale, MN), “Selfaligning optical micro-mechanical device package,” August 3, 2004. Saia, Richard Joseph (Niskayuna, NY), Durocher, Kevin Matthew (Waterford, NY), Kapusta, Christopher James (Duanesburg, NY), Nielsen, Matthew Christian (Schenectady, NY), “Microelectromechanical system device packaging method,” July 27, 2004. Furuyama, Hideto (Kanagawa-ken, JP), “Optical wiring device,” July 6, 2004. Stark, David H. (Evergreen, CO), “Hermetically sealed micro-device package with window,” July 6, 2004. Stark, David H. (Evergreen, CO), “Hermetically sealed micro-device package using cold-gas dynamic spray material deposition,” April 20, 2004. Shih, Wu-Sheng (Rolla, MO), Lamb, III, James E. (Rolla, MO), Daffron, Mark (Rolla, MO), “Contact planarization materials that generate no volatile byproducts or residue during curing,” April 6, 2004. Margomenos, Alexandros (Ann Arbor, MI), Herrick, Katherine J. (Westford, MA), Becker, James P. (Bozeman, MT), Katehi, Linda P. B. (Northville, MI), “On-wafer packaging for RFMEMS,” February 24, 2004. Chinthakindi, Anil K. (Fishkill, NY), Groves, Robert A. (Highland, NY), Stein, Kenneth J. (Sandy Hook, CT), Subbanna, Seshadri (Brewster, NY), Volant, Richard P. (New Fairfield, CT), “Microelectromechanical varactor with enhanced tuning range,” February 24, 2004. Chinthakindi, Anil K. (Poughkeepsie, NY), Groves, Robert A. (Highland, NY), Stein, Kenneth J. (Sandy Hook, CT), Subbanna, Seshadri (Brewster, NY), Volant, Richard P. (New Fairfield, CT), “Micro-electromechanical varactor with enhanced tuning range,” December 9, 2003.
19
20
Chapter One 6,643,065
6,639,313
6,635,509 6,627,814
6,624,003
6,580,858
6,535,685
6,516,131
6,516,104 6,481,570
6,455,878
6,400,009
6,379,988
Silberman, Donn Michael (Aliso Viejo, CA), “Variable spacing diffraction grating,” November 4, 2003. Martin, John R. (Foxborough, MA), Harney, Kieran H. (Andover, MA), “Hermetic seals for large optical packages and the like,” October 28, 2003. Ouellet, Luc (Granby, CA), “Wafer-level MEMS packaging,” October 21, 2003. Stark, David H. (Evergreen, CO), “Hermetically sealed micro-device package with window,” September 30, 2003. Rice, Janet L. (Round Rock, TX), “Integrated MEMS device and package,” September 23, 2003. Chen, Jingkuang (Rochester, NY), Kubby, Joel A. (Rochester, NY), Sun, Decai (Los Altos, CA), “Micro-opto-electro-mechanical system (MOEMS),” June 17, 2003. Tullis, Barclay J. (Palo Alto, CA), “Arcuate fiber routing using stepped grooves,” March 18, 2003. Tullis, Barclay J. (Palo Alto, CA), “Structures and methods for aligning fibers,” February 4, 2003. Furuyama, Hideto (Kanagawa-ken, JP), “Optical wiring device,” February 4, 2003. Henshall, Gordon D (Harlow, GB), Rolt, Stephen (Herts, GB), “Packaging atmosphere and method of packaging a MEMS device,” November 19, 2002. Bhat, Jerome Chandra (San Francisco, CA), Ludowise, Michael Joseph (San Jose, CA), Steigerwald, Daniel Alexander (Cupertino, CA), “Semiconductor LED flip-chip having low refractive index underfill,” September 24, 2002. Bishop, David John (Summit, NJ), Gates, II, John VanAtta (New Providence, NJ), Kim, Jungsang (Basking Ridge, NJ), “Hermatic firewall for MEMS packaging in flip-chip bonded geometry,” June 4, 2002. Peterson, Kenneth A. (Albuquerque, NM), Conley, William R. (Tijeras, NM), “Pre-release plastic packaging of MEMS and IMEMS devices,” April 30, 2002.
Introduction to MEMS 6,335,224
6,297,072
1.6.2
Peterson, Kenneth A. (Albuquerque, NM), Conley, William R. (Tijeras, NM), “Protection of microelectronic devices during packaging,” January 1, 2002. Tilmans, Hendrikus A. C. (Maastricht, NL), Beyne, Eric (Leuven, BE), Van de Peer, Myriam (Brussel, BE), “Method of fabrication of a microstructure having an internal cavity,” October 2, 2001.
Japanese MEMS Packaging Patents
Some of the Japanese MEMS packaging patents selected from the Japan Patent Office (JPO) since 2001 are as follows: Patent No. 2008-298950 2008-244442
2008-229823 2008-221450
2008-211124 2008-209616
2008-198607
2008-193544
2008-185723 2008-185621
Owner(s)/Title/Date Yokoi, Junichi, “Optical scanning apparatus,” 11.12.2008. Seppala, Bryan R., Curtis, Harlan L., DCamp, Jon B., Spielberger, Richard K., “System and method for sealing MEMS device,” 09.10.2008. Aoki, Toshihiko, “Manufacturing method of MEMS device,” 02.10.2008. Fujii, Yoshio, Ogawa, Shinpei, Yokoyama, Yoshinori, Endo, Kazuyo, “MEMS package and manufacturing method therefor,” 25.09.2008. Chino, Mitsuru, “Semiconductor device storing package,” 11.09.2008. Kato, Seiichi, Nanjo, Takeshi, Otaka, Koichi, “Optical deflector and method of manufacturing the same,” 11.09.2008. Arthur, Stephen D., Elasser, Ahmed, Wright, Joshua Isaac, Subramanian, Kanakasabapathi, Keimel, Christopher Fred, Gowda, Arun Virupaksha, “Power overlay structure for MEM device, and method for producing power overlay structure for MEM device,” 28.08.2008. Aoki, Nobuhisa, Takano, Takeshi, Miyashita, Takumi, “Amplifier which takes internal matching according to signal characteristic,” 21.08.2008. Yokoi, Junichi, Sakai, Toshio, “Optical scanner,” 14.08.2008. Fujino, Hitoshi, Sakai, Toshio, “Optical deflector,” 14.08.2008.
21
22
Chapter One 2008-182103 2008-132587
2008-105162 2008-091334
2008-047955
2007-331099
2007-331098
2007-281292 2007-245339
2007-221105 2007-218902 2007-214440 2007-214439 2007-203451 2007-155714 2007-144617 2007-136668
Hatakeyama, Tomoyuki, “Airtight seal package,” 07.08.2008. Eskridge, Mark H., Jafri, Ijaz H., “Method of manufacturing wafer-level vacuum packaged device,” 12.06.2008. Hata, Shohei, Sakamoto, Eiji, Matsushima, Naoki, “Functional element,” 08.05.2008. Manuel, Carmona Flores, Kihara, Tatsuji, Jaume, Esteve Tinto, “MEMS package, and manufacturing method therefore, as well as integrated circuit including MEMS package,” 17.04.2008. Tenmyo, Hiroyuki, Isada, Naoya, Matsumoto, Kunio, Watanabe, Kazushi, Nagashima, Shiro, “Packaging structure having three-dimensional wiring,” 28.02.2008. Pyo, Sung-gyu, Kim, Dong-joon, “Package for MEMS element, and method for manufacturing the same,” 27.12.2007. Kim, Dong-joon, Pyo, Sung-gyu, “Package of MEMS device and method for manufacturing the same,” 27.12.2007. Ohara, Satoshi, “Semiconductor device mounting structure,” 25.10.2007. Robert, Philippe, “Microelectronic composite, especially packaging structure in sealing cavity of MEMS,” 27.09.2007. Eskridge, Mark H., “Sealing of MEMS device using liquid crystal polymer,” 30.08.2007. Eskridge, Mark H., “Discrete stress isolator,” 30.08.2007. Kuramochi, Satoru, Fukuoka, Yoshitaka, “Electronic device,” 23.08.2007. Satoru, Kuramochi and Yoshitaka, Fukuoka, “Composite sensor package,” 23.08.2007. MacGugan, Douglas C., “Integrated MEMS package,” 16.08.2007. MacGugan, Douglas C., “Compact package for moving sensor sensing axis,” 21.06.2007. D’Camp, Jon B., Curtis, Harlan L., “MEMS device packaging method,” 14.06.2007. D’Camp, Jon B., Curtis, Harlan L., “MEMS flipchip packaging,” 07.06.2007.
Introduction to MEMS 2007-132687 2007-124500
2007-108753
2007-088189
2007-082233 2007-060661
2007-042786 2007-017199
2006-321016 2006-286794 2006-270045
2006-247833
2006-202909
Taniguchi, Hajime, “Package for sensor, and detector using the same,” 31.05.2007. Yoshida, Koichi, Yamada, Toru, Kojima, Hideki, Makihata, Katsuhiro, “Acoustic sensor and method for manufacturing acoustic sensor,” 17.05.2007. Park, Heung-woo, Lee, Yeong-gyu, Boku, Shoshu, Lim, Ohk-kun, Park, Dong-hyun, “MEMS package and optical modulator module package,” 26.04.2007. Tenmyo, Hiroyuki, Isada, Naoya, Isobe, Atsushi, Terano, Akihisa, Matsumoto, Kunio, Ite, Mayumi, “MEMS (micro electronic mechanical system) package and its manufacturing method,” 05.04.2007. So, Seitan, “Silicon capacitor microphone and method for packaging same,” 29.03.2007. So, Seitan, “Silicon based condenser microphone and packaging method for the same,” 08.03.2007. Oya, Yoichi, “Micro device and its packaging method,” 15.02.2007. Tokushige, Nobuaki, Naka, Toshio, “Chip scale package and its manufacturing method,” 25.01.2007. Yoshikawa, Yasuhiro, Tajiri, Hiroyuki, “MEMS package,” 30.11.2006. Takahashi, Norio, “Semiconductor chip package and its manufacturing method,” 19.10.2006. Lim, Chang Hyun, Hwang, Woong Lin, Choi, Seog Moon, Park, Ho Joon, Lee, Sung Jun, Choi, Sang Hyun, “Light emitting diode package having electrostatic discharge protection functionality,” 05.10.2006. Kim, Jong-seok, Kim, Duck-hwan, Nam, Kuang-woo, Park, Yun-kwon, Yun, Seok-chul, Choa, Sung-hoon, So, Inso, “MEMS element package and its manufacturing method,” 21.09.2006. Ikeuchi, Naoki, Hashimoto, Hiroyuki, “Semiconductor device having minute structure and method of manufacturing minute structure,” 03.08.2006.
23
24
Chapter One 2006-190804
2006-186376
2006-186362
2006-173599
2006-173598
2006-147995
2006-123160
2006-121052
2006-121043
2006-119603
2006-099107
2006-099096
Kodate, Junichi, Machida, Katsuyuki, Urano, Masami, “Semiconductor device and its manufacturing method,” 20.07.2006. Kim, Jong-seok, Park, Yun-kwon, So, Inso, Kim, Duck-hwan, Nam, Kuang-woo, Yun, Seok-chul, “MEMS element and its manufacturing method,” 13.07.2006. Kim, Jong-seok, Park, Yun-kwon, So, Inso, Nam, Kuang-woo, Yun, Seok-chul, “MEMS element package and its manufacturing method,” 13.07.2006. Fazzio, Ronald S., Dungan, Thomas E., “Integrated wafer package of micro electrical machine and active device circuit,” 29.06.2006. Dungan, Thomas E., Fazzio, Ronald S., “Single integrated wafer package and assembling method of wafer package,” 29.06.2006. Kodate, Junichi, Machida, Katsuyuki, Urano, Masami, Kuwabara, Hiroshi, Terada, Jun, “Variable capacitance element and manufacturing method thereof,” 08.06.2006. Palmateer, Lauren, Gally, Brian J., Cummings, William J., “Method and device for providing MEMS device package having secondary seal,” 18.05.2006. Palmateer, Lauren, Cummings, William J., Gally, Brian J., Chui, Clarence, Kothari, Manish, “Method and system for packaging MEMS device together with incorporated getter,” 11.05.2006. Palmateer, Lauren, Cummings, William J., Gally, Brian J., Sampsell, Jeffrey B., “System and method for display provided with activated desiccant,” 11.05.2006. Gally, Brian J., Palmateer, Lauren, Cummings, William J., “System and method for protecting microelectromechanical system using backplate with non-flat portion,” 11.05.2006. Palmateer, Lauren, “System and method for display device with end-of-life phenomenon,” 13.04.2006. Floyd, Philip D., Arbuckle, Brian W., “Device having patterned spacer for backplate and method of making the same,” 13.04.2006.
Introduction to MEMS 2006-091849
2006-003277
2005-332957 2005-329532
2005-276816
2005-250307 2005-166909 2005-109221
2005-040940
2005-034987 2005-019966
2005-018015
2004-322157
2004-235465 2004-160654
Miles, Mark W., Sampsell, Jeffrey B., Palmateer, Lauren, Arbuckle, Brian W., Floyd, Philip D., “Method and system to package MEMS device,” 06.04.2006. Kanno, Yoshinori, “Semiconductor acceleration sensor system and its manufacturing method,” 05.01.2006. Okamoto, Kazuhisa, “Package manufacturing method,” 02.12.2005. Hong, Suk-kee, Lee, Yeong-gyu, Park, Heungwoo, “MEMS package having side seal member and its manufacturing method,” 02.12.2005. Tsui, Kenneth, Geisberger, Aaron, Skidmore, George, “Micro connector and non-powered microassembly with micro connector,” 06.10.2005. Hara, Koichi, “Optical deflector,” 15.09.2005. Yamamoto, Satoshi, Suemasu, Tatsuo, “Package and its manufacturing method,” 23.06.2005. Kawakubo, Takashi, Yasumoto, Yasuaki, Itaya, Kazuhiko, “Wafer-level package and its manufacturing method,” 21.04.2005. Snyder, Tanya Jegeris, Yi, Robert H., Wilson, Robert Edward, “Wafer bonding method using reactive foils for massively parallel micro-electromechanical systems packaging,” 17.02.2005. Smith, Mark A., Boucher, William R., Haluzak, Charles C., “Fluidic MEMS device,” 10.02.2005. Ikeda, Osamu, Okoda, Toshiyuki, “Semiconductor device and method of manufacturing the same,” 20.01.2005. Lee, Hyun Kee, Jung, Sung Cheon, Hong, Yoon Shik, “Optical switch and manufacturing method thereof,” 20.01.2005. Hino, Atsushi, Matsumura, Takeshi, “Working method for work and tacky adhesive sheet used for the same,” 18.11.2004. Yuasa, Mitsuhiro, “Bonding method, bonding device and sealant,” 19.08.2004. Lee, Eun-sung, Koh, Byeong-cheon, Moon, Chang-youl, Chun, Kuk Jin, “Side-bonding method for flip chip system in semiconductor device, MEMS device package and package method using the same,” 10.06.2004.
25
26
Chapter One 2004-160649
2004-158665
2004-136435
2003-347357 2003-297876
2003-243550
2003-075741
2002-246489
2002-236266
2002-043463
2002-043449
2001-196484
2001-185635
Lee, Moon-chul, Jun, Chan-bong, Choi, Hyung, Jung, Kyu-dong, Jang, Mi, Hong, Seog-woo, Kang, Seok-jin, Chung, Seok-whan, “Forming method of via hole of glass wafer,” 10.06.2004. Usami, Akira, Ohashi, Hidemasa, Nishino, Tamotsu, Owada, Satoru, Maeda, Chisako, Yoshida, Yukihisa, “Substrate for package and its manufacturing method,” 03.06.2004. Song, Ci-moo, Kang, Seok-jin, Chung, Seokwhan, Lee, Moon-chul, Jung, Kyu-dong, Kim, Jong-seok, Jun, Chan-bong, Hong, Seog-woo, Kang, Jung-ho, “Method of metal wiring for undercut,” 13.05.2004. Kawaguchi, Hitoshi, “Manufacturing method of semiconductor package,” 05.12.2003. Kawaguchi, Hitoshi, Takahashi, Toyomasa, “Manufacturing method for semiconductor package,” 17.10.2003. Kim, Woon-bae, Shin, Keisai, Cho, Soko, Kang, Seung-goo, “Hermetic sealing method for oxidation prevention at low temperature,” 29.08.2003. Boie, Robert Albert, Kim, Yunsang, Soh, Hyongsok, “Constitution of MEMS driver circuit,” 12.03.2003. Cho, Chang-ho, Shin, Hyung-jae, Kim, Woonbae, “Wafer level hermetic sealing method,” 30.08.2002. Jin, Sungho, Soh, Hyongsok, “Magnetically packaged optical MEMS device and method for making the same,” 23.08.2002. Kang, Seok-jin, “Surface mounting type chip scale packaging method of electronic and MEMS element,” 08.02.2002. Degani, Yinon, Dudderar, Thomas D., Tai, King L., “Micro mechanical packaging apparatus,” 08.02.2002. Ha, Byeoung Ju, Baek, Seog-soon, Kim, Hyunchul, Song, Hoon, Oh, Yong-soo, “Manufacturing method of MEMS structure enabling wafer level vacuum packaging,” 19.07.2001. Bishop, David John, Gates, John Vanatta, Kim, Jungsang, “Package having cavity for housing MEMS,” 06.07.2001.
Introduction to MEMS 2001-144117
Oakatto, John W., Downa, Andrew Steven, Rin, Tsuen Fwan, “Improved MEMS wafer-level package,” 25.05.2001.
1.6.3 Worldwide MEMS Packaging Patents Some of the MEMS packaging patents selected from European Patent Office (EPO) since 2002 are as follows: Title/Owner(s)/Patent No./Date 1. “Wafer level chip size package for MEMS devices and method for fabricating the same,” Wang, Zhiqi (CN), Yu, Guoqing (CN) (+2), US2009057868 (A1)—2009-03-05. 2. “Method for packaging an optical MEMS device,” Khonsari, Nassim (US), Chui, Clarence (US), EP2029473 (A2)—200903-04. 3. “Patterned contact sheet to protect critical surfaces in manufacturing processes,” Ya, Michael Wang Qing (US), Zhang, Junhong (US), CN101323428 (A)—2008-12-17. 4. “Vertically integrated 3-axis MEMS accelerometer with electronics,” Nasiri, Steven S. (US), Seeger, Joseph (US) (+1), US2008314147 (A1)—2008-12-25. 5. “Mirror and mirror layer for optical modulator and method,” Chui, Clarence (US), Sampsell, Jeffrey B. (US), US2008314866 (A1)—2008-12-25. 6. “System and method of fabricating micro cavities,” Wan, Chang-Feng (US), US2008308920 (A1)—2008-12-18. 7. “Electronic device comprising a MEMS element,” Dekker, Ronald (NL), Polhmann, Hauke (NL) (+1), CN101309854 (A)—2008-11-19. 8. “Apparatus for downhole fluids analysis utilizing micro electro mechanical systems (MEMS) or other sensors,” Terabayashi, Toru (VG), Sugimoto, Tsutomu (VG) (+3), CN101309853 (A)— 2008-11-19. 9. “MEMS device vacuum encapsulation method,” Jin, Yufeng (CN), Zhang, Yangfei (CN) (+2), CN101301993 (A)—2008-11-12. 10. “Packaging body and packaging component for microphone of micro electro-mechanical systems,” Huang, Zhaoda (CN), Jian, Xintang (CN), CN101316462 (A)—2008-12-03. 11. “Packaging body and packaging component for microphone of micro electro-mechanical systems,” Huang, Zhaoda (CN), Jian, Xintang (CN), CN101316461 (A)—2008-12-03. 12. “Packaging of Mems devices,” Johnson, Donald W. (US), Nagale, Milind P. (US), EP1997128 (A2)—2008-12-03.
27
28
Chapter One 13. “Silicon microphone with improved structure,” Wang, Xianbin (CN), Dang, Maoqiang (CN) (+2), CN201138866 (Y)—2008-10-22. 14. “Package and packaging assembly of microelectromechanical sysyem microphone,” Huang, Chao-Ta (TW), Chien, Hsin-Tang (TW), US2008283988 (A1)—2008-11-20. 15. “Package and packaging assembly of microelectromechanical sysyem microphone,” Huang, Chao-Ta (TW), Chien, Hsin-Tang (TW), US2008283942 (A1)—2008-11-20. 16. “Capacitance type micro-accelerometer,” Liu, Minjie (CN), Liu, Yunfeng (CN) (+2), CN101271125 (A)—2008-09-24. 17. “Silicon piezoresistance type pressure transducer encapsulation structure based on substrates,” Wang, Yuelin (CN), Wu, Yanhong (CN) (+2), CN101271029 (A)—2008-09-24. 18. “MEMS device support structure for sensor packaging,” Ahmad, Nazir (US), US2008277747 (A1)—2008-11-13. 19. “MEMS device with integral packaging,” Cohn, Michael B. (US), Xu, Ji-Hai (US), US2008272867 (A1)—2008-11-06. 20. “Packaged MEMS device assembly,” Haluzak, Charles C. (US), Pollard, Jeffrey R. (US) (+5), US2008272446 (A1)—2008-11-06. 21. “MEMS device airtightness packaging method,” Chen, Jing (CN), Wu, Yexian (CN) (+1), CN101234745 (A)—2008-08-06. 22. “Orientation-dependent etching of deposited AIN for structural use and sacrificial layers in MEMS,” Bouche, Guillaume (US), Wall, Ralph N. (US), US2008268575 (A1)—2008-10-30. 23. “Packaging a MEMS device using a frame,” Natarajan, Bangalore R. (US), EP1979268 (A2)—2008-10-15. 24. “Microelectromechanical systems, and methods for encapsualting and fabricating same,” Partridge, Aaron (US), Lutz, Markus (US) (+1), US2008237756 (A1)—2008-10-02. 25. “Functional device,” Hata, Shohei (JP), Sakamoto, Eiji (JP) (+1), US2008233349 (A1)—2008-09-25. 26. “Power overlay structure for MEM device, and method for producing power overlay structure for MEM device,” Arthur, Stephen D., Elasser, Ahmed (+4), JP2008198607 (A)—200808-28. 27. “MEMS fiber optic microphone,” Chin, Ken K. (US), Feng, Guanhua (US) (+1), WO2008100266 (A2)—2008-08-21. 28. “Apparatus for driving micromechanical devices,” Miles, Mark W. (US), US2008191978 (A1)—2008-08-14.
Introduction to MEMS 29. “Method for manufacturing a semiconductor package structure having micro-electro-mechanical systems,” Wang, MengJen (TW), Yang, Hsueh-An (TW), US2008188026 (A1)—200808-07. 30. “Package and method for making the same,” Wang, MengJen (TW), US2008185706 (A1)—2008-08-07. 31. “Methods and systems for wafer level packaging of MEMS structures,” Yang, Xiao (US), Payne, Justin (US) (+3), WO2008085779 (A1)—2008-07-17. 32. “Design of MEMS packaging,” Kvisteroy, Terje (NO), Westby, Eskild (NO), US2008164546 (A1)—2008-07-10. 33. “Packaging structure and method of a MEMS microphone,” Hsiao, Wei-Min (TW), US2008166000 (A1)—2008-07-10. 34. “MEMS packaging with reduced mechanical strain,” Kvisteroy, Terje (NO), Westby, Eskild (NO), EP1944266 (A1)—2008-07-16. 35. “Packaging of Micro Devices,” O’Mahony, Conor (IE), Hill, Martin (IE), US2008145976 (A1)—2008-06-19. 36. “High-aspect-ratio metal-polymer composite structures for nano interconnects,” Aggarwal, Ankur (US), Raj, Pulugurtha Markondeya (US) (+1), US2008136035 (A1)—2008-06-12. 37. “MEMS package and packaging method thereof,” Jung, Sung-Hae (KR), Lee, Myung-Lae (KR) (+4), WO2008069394 (A1)—2008-06-12. 38. “Integrated thermal systems,” Henderson, H. Thurman (US), Shuja, Ahmed (US) (+3), US2008128898 (A1)—2008-06-05. 39. “Microelectromechanical devices and fabrication methods,” Metz, Matthias (US), Pan, Zhiyu (CN) (+3), WO2008067097 (A2)—2008-06-05. 40. “Hermetically sealed wafer level packaging for optical MEMS devices,” Yang, Xiao (US), CN101183675 (A)—2008-05-21. 41. “Polymer object optical fabrication process,” Cregger, Robert Brian (US), WO2008063433 (A2)—2008-05-29. 42. “X-Y axis dual-mass tuning fork gyroscope with vertically integrated electronics and wafer-scale hermetic packaging,” Seeger, Joseph (US), Nasiri, Steven S. (US) (+1), US2008115579 (A1)—2008-05-22. 43. “MEMS package, and manufacturing method therefore, as well as integrated circuit including MEMS package,” Manuel, Carmona Flores, Kihara, Tatsuji (+1), JP2008091334 (A)— 2008-04-17.
29
30
Chapter One 44. “Microelectronic flow sensor packaging method and system,” Ricks, Lamar F. (US), WO2008057911 (A2)—2008-05-15. 45. “Hermetically sealed wafer level packaging for optical MEMS devices,” Yang, Xiao (US), GB2443352 (A)—2008-04-30. 46. “Methods for depositing, releasing and packaging microelectromechanical devices on wafer substrates,” Patel, Satayadev R. (US), Huibers, Andrew G. (US) (+8), US2008096313 (A1)—2008-04-24. 47. “Package structure and packaging method of MEMS microphone,” Chen, Jung-Tai (TW), Chu, Chun-Hsun (TW), US2008083960 (A1)—2008-04-10. 48. “Laser assisted system and method for bonding of surfaces,” Wang, Changhai (GB), Hand, Duncan (GB) (+1), EP1907160 (A1)—2008-04-09. 49. “Method for preparing spherical glass micro-cavity used for MEMS disc type packaging,” Shang, Jintang (CN), Huang, Qingan (CN) (+2), CN101143702 (A)—2008-03-19. 50. “Chip packaging systems and methods,” D’Camp, Jon B. (US), Curtis, Harlan L. (US) (+2), US2008063505 (A1)—2008-03-13. 51. “Micro electro-mechanical system module package,” Yen, Tzu-Yin (TW), Yeh, Cung-Mao (TW), US2008061409 (A1)— 2008-03-13. 52. “Integrated MEMS packaging,” Lu, Jun (CA), Menard, Stephane (CA), WO2008034233 (A1)—2008-03-27. 53. “Packaging structure having three-dimensional wiring,” Tenmyo, Hiroyuki, Isada, Naoya (+3), JP2008047955 (A)— 2008-02-28. 54. “MEMS fiber optic microphone,” Chin, Ken K. (US), Feng, Guanhua (US) (+1), US2008049230 (A1)—2008-02-28. 55. “MEMS packaging with improved reaction to temperature changes,” Strei, David (US), CN101098825 (A)—2008-01-02. 56. “Method and system for sealing packages for optics,” Yang, Xiao (US), Chen, Dongmin (US), US2008014682 (A1)—200801-17. 57. “MEMS microphone packaging structure,” Pan, Zhengmin (CN), CN200994191 (Y)—2007-12-19. 58. “Multiple internal seal ring micro-electro-mechanical system vacuum packaging method,” Hayworth, Ken J. (US), Yee, Karl Y. (US) (+5), US2007298542 (A1)—2007-12-27. 59. “Method for forming a hermetically sealed cavity,” Witvrouw, Ann (BE), Rico, Raquel H. (ES) (+1), US2007298238 (A1)—200712-27.
Introduction to MEMS 60. “Stacked die package for MEMS resonator system,” Gupta, Pavan (US), Razda, Eric (US), US2007290364 (A1)—2007-12-20. 61. “Hermetically sealed wafer level packaging for optical MEMS devices,” Yang, Xiao (US), GB2439403 (A)—2007-12-27. 62. “Method for manufacturing plastic packaging of MEMS devices and structure thereof,” Chen, Jung Tai (TW), Chang, Wen Yang (TW) (+2), KR20070095756 (A)—2007-10-01. 63. “MEMS device packaging methods,” D’Camp, Jon B., Curtis, Harlan L., SG132639 (A1)—2007-06-28. 64. “MEMS flip-chip packaging,” D’Camp, Jon B. (US), Curtis, Harlan L. (US), SG132638 (A1)—2007-06-28. 65. “Condenser microphone and packaging method for the same,” Song, Chung-Dam, SG131039 (A1)—2007-04-26. 66. “Silicon based condenser microphone and packaging method for the same,” Song, Chung-Dam, SG130158 (A1)—2007-03-20. 67. “Desiccant in a MEMS device,” Palmateer, Lauren (US), WO2007136706 (A1)—2007-11-29. 68. “Semiconductor device having microstructure and method of manufacturing microstructure,” Ikeuchi, Naoki (JP), Hashimoto, Hiroyuki (JP), US2007262306 (A1)—2007-11-15. 69. “High performance MEMS packaging archetecture,” Lafond, Peter H. (US), Yu, Lianzhong (US), EP1853928 (A1)—2007-11-14. 70. “Contact planarization materials that generate no volatile byproducts or residue during curing,” Shih, Wu-Sheng (TW), Lamb, James E. III (US) (+1), TW278488 (B)—2007-04-11. 71. “Packaging structure of MEMS microphone,” Park, Peter (KR), Choo, Yun-Jai (KR) (+1), WO2007123300 (A1)—2007-11-01. 72. “Packaging structure of MEMS microphone,” Choo, Yunjai (KR), Park, Peter (KR), WO2007123293 (A1)—2007-11-01. 73. “Method and system for packaging a MEMS device,” Miles, Mark W. (US), Sampsell, Jeffrey B. (US), US2007247693 (A1)— 2007-10-25. 74. “Packaging a MEMS device using a frame,” Natarajan, Bangalore R. (US), Palmateer, Lauren (US), US2007242345 (A1)— 2007-10-18. 75. “MEMS devices and processes for packaging such devices,” Natarajan, Bangalore R. (US), Ganti, Surya (US), US2007242341 (A1)—2007-10-18. 76. “Microelectronic composite, especially packaging structure in sealing cavity of MEMS,” Robert, Philippe, JP2007245339 (A)—2007-09-27.
31
32
Chapter One 77. “Surface coating for electronic systems,” Cho, Junghyun (US), Oliver, Scott (US) (+2), US7282254 (B1)—2007-10-16. 78. “Self-packaging MEMS device,” Heck, John (US), US2007235501 (A1)—2007-10-11. 79. “Multi-unit planar lightwave circuit wavelength dispersive device,” Colbourne, Paul (CA), CA2584147 (A1)—2007-10-06. 80. “Packaging structure of MEMS microphone,” Park, Sung Ho (KR), Lim, Jun (KR) (+1), KR100737726 (B1)—2007-07-04. 81. “Packaging structure of MEMS microphone and construction method thereof,” Choo, Yun Jai (KR), Park, Peter (KR) (+1), KR100737728 (B1)—2007-07-04. 82. “Method of packaging of MEMS device at the vacuum state using a silicide bonding,” Lee, Ho Young (KR), Cho, Sung Woo (KR), KR20070078239 (A)—2007-07-31. 83. “Method of packaging of MEMS device at the vacuum state using a silicide bonding and vacuum packaged MEMS device using the same,” Lee, Ho Young (KR), Cho, Sung Woo (KR), KR20070078233 (A)—2007-07-31. 84. “Microstructure sealing tool and methods of using the same,” Schaadt, Gregory P. (US), US2007172991 (A1)—2007-07-26. 85. “Systems and methods of controlling micro-electromechanical devices,” Miles, Mark W. (US), US2007146376 (A1)—200706-28. 86. “Method for singulating a released microelectromechanical system wafer,” Loeppert, Peter V. (US), WO2007081346 (A1)— 2007-07-19. 87. “Micro-electro-mechanical systems (MEMS) device and system and method of producing the same,” Bar-Sadeh, Eyal (IL), Talalaevski, Alexander (IL) (+1), TW267490 (B)—2006-12-01. 88. “MEMS module package and packaging method,” Lee, Yeong Gyu (KR), KR20070042244 (A)—2007-04-23. 89. “MEMS device package and packaging method,” Kim, Dae Jun (KR), Lee, Yeong Gyu (KR) (+1), KR20070040472 (A)— 2007-04-17. 90. “MEMS device package and packaging method,” Kim, Dae Jun (KR), Lee, Yeong Gyu (KR) (+1), KR20070040471 (A)— 2007-04-17. 91. “MEMS module and packaging method,” Lee, Yeong Gyu (KR), KR20070040033 (A)—2007-04-16. 92. “Method for adjusting the frequency of a MEMS resonator,” Lutz, Aaron, Partridge, Markus (DE), CN1977448 (A)—200706-06.
Introduction to MEMS 93. “Micro electro-mechanical system packaging and interconnect,” Chen, Chien-Hua (US), Bamber, John (US) (+1), US2007128828 (A1)—2007-06-07. 94. “Wafer level packaging process,” Sridhar, Uppili (US), Zou, Quanbo (US), WO2007055924 (A2)—2007-05-18. 95. “Miniature package for translation of sensor sense axis,” MacGugan, Douglas C. (US), EP1785392 (A2)—2007-05-16. 96. “Method for integrated MEMS packaging,” Hartzell, John W. (US), Walton, Harry G. (GB) (+1), US2007099327 (A1)—200705-03. 97. “Systems and methods of testing micro-electromechanical devices,” Miles, Mark W. (US), US2007097134 (A1)—2007-05-03. 98. “Microphone and manufacturing method thereof,” Jang, Jau-Jr (TW), Tsai, Tzuen-Yi (TW) (+1), TW262735 (B)—2006-09-21. 99. “MEMS (micro electronic mechanical system) package and its manufacturing method,” Tenmyo, Hiroyuki, Isada, Naoya (+4), JP2007088189 (A)—2007-04-05. 100. “Micro electromechanical system chip size airtight packaging vertical interconnecting structure and its manufacturing method,” Wang, Yuchuan Luo (CN), CN1935630 (A)—200703-28. 101. “MEMS package and method of forming the same,” McBean, Ronald V. (US), WO2007027380 (A2)—2007-03-08. 102. “Micro device and its packaging method,” Oya, Yoichi, JP2007042786 (A)—2007-02-15. 103. “Microelectromechanical devices and fabrication methods,” Yama, Gary (US), US2007042521 (A1)—2007-02-22. 104. “Chip scale package and its manufacturing method,” Tokushige, Nobuaki, Naka, Toshio, JP2007017199 (A)—2007-01-25. 105. “MEMS micro high sensitivity magnetic field sensor and manufacturing method,” Liu, Wu Yaming (CN), CN1912646 (A)—2007-02-14. 106. “Silicon based condenser microphone and packaging method for the same,” Song, Chung-Dam (KR), WO2007015593 (A1)— 2007-02-08. 107. “MEMS packaging method for enhanced EMI immunity using flexible substrates,” Wang, Zhe (SG), Miao, Yubo (SG), US2007013052 (A1)—2007-01-18. 108. “Method of making an X-Y axis dual-mass tuning fork gyroscope with vertically integrated electronics and wafer-scale hermetic packaging,” Nasiri, Steven S. (US), Flannery, Anthony F., Jr. (US), US2007012653 (A1)—2007-01-18.
33
34
Chapter One 109. “Method and system for packaging MEMS devices with incorporated getter,” Palmateer, Lauren (US), Cummings, William J. (US) (+3), KR20060092914 (A)—2006-08-23. 110. “Methods for depositing, releasing and packaging microelectromechanical devices on wafer substrates,” Patel, Satyadev R. (US), Huibers, Andrew G. (US) (+1), US2007001247 (A1)—2007-01-04. 111. “Two-freedom air-floated precisely locating platform for IC packaging,” Zhang, Dawei (CN), CN1887686 (A)—2007-01-03. 112. “MEMS package,” Yoshikawa, Yasuhiro, Tajiri, Hiroyuki, JP2006321016 (A)—2006-11-30. 113. “Encapsulation process for microelectromechanical structures,” Dudley, Bruce W., Wood, Robert L., KR20010051498 (A)—200106-25. 114. “Method of packaging MEMS,” Ouellet, Luc (CA), Chowdhury, Mamur (CA), EP1734001 (A2)—2006-12-20. 115. “Display device having a movable structure for modulating light and method thereof,” Miles, Mark W. (US), US2006274074 (A1)—2006-12-07. 116. “Production method of glass penetrating wiring board, glass penetrating wiring board, and probe card and packaging element using glass penetrating wiring board,” Fujimoto, Satoshi (JP), WO2006129848 (A1)—2006-12-07. 117. “X-Y axis dual-mass tuning fork gyroscope with vertically integrated electronics and wafer-scale hermetic packaging,” Nasiri, Steve S. (US), Seeger, Joseph (US), TW247896 (B)— 2006-01-21. 118. “Packaging method for rf mems switch to minimize short of switch connection,” Lee, Gyu Bok, KR20040093807 (A)—200411-09. 119. “Bonding method of flip-chip manner for semiconductor apparatus in lateral bonded type, MEMS package using the same, and packaging method,” Jin, Jun Guk, Cheon, Ko Byeong (+2), KR20040042924 (A)—2004-05-22. 120. “Method for forming via hole of glass wafer,” Choi, Hyeong, Hong, Seok U. (+6), KR20040042003 (A)—2004-05-20. 121. “Metal line method even though it has undercut,” Hong, Seok U., Jun, Chan Bong (+7), KR20040034949 (A)—200404-29. 122. “MEMS switch and method for packaging the same,” Lee, Dae Sung (KR), Sung, Woo Kyung (KR) (+3), KR20050113340 (A)—2005-12-02.
Introduction to MEMS 123. “Method of packaging of MEMS device at the vacuum state and vacuum packaged MEMS device using the same,” Lee, Ho Young (KR), Kim, Yong Hyup (KR) (+3), KR20050100039 (A)—2005-10-18. 124. “Electronic parts packaging structure and method of manufacturing the same,” Sunohara, Masahiro (JP), Higashi, Mitsutoshi (JP), US2006246630 (A1)—2006-11-02. 125. “Apparatus for packaging MEMS element and method thereof,” Jang, Hyuk Kyoo (KR), Noh, Seung Jeong (KR) (+3), KR20060061044 (A)—2006-06-07. 126. “Pizoelectric rf MEMS switch using wafer unit packaging and microfabrication technology and fabrication method thereof,” Park, Jae Hyoung (KR), Lee, Hee Chul (KR) (+1), KR20060022561 (A)—2006-03-10. 127. “Method for manufacturing structure of micro electromechanical system capable of wafer-level vacuum packaging,” Baek, Seok Sun (KR), Ha, Byeong Ju (KR) (+3), KR20010045332 (A)—2001-06-05. 128. “Variable display,” Jensen, Thomas (US), Lawler, Casimer E., Jr. (US), US2006227002 (A1)—2006-10-12. 129. “MEMS packaging structure and methods,” Haluzak, Charles C. (US), Pollard, Jeffrey R. (US), US2006228869 (A1)—200610-12. 130. “Reactive nano-layer material for MEMS packaging,” Lu, Daoqiang (US), Heck, John (US), US2006220223 (A1)—200610-05. 131. “Method of fabrication of AI/GE bonding in a wafer packaging environment and a product produced therefrom,” Nasiri, Steven S. (US), Flannery, Anthony Francis, Jr. (US), WO2006101769 (A2)—2006-09-28. 132. “Structure and process for packaging RF MEMS and other devices,” Schaper, Leonard W. (US), Malshe, Ajay P. (US) (+1), US2006211177 (A1)—2006-09-21. 133. “Passive devices and modules for transceiver and manufacturing method thereof,” Song, In Sang (KR), KR20020095728 (A)—2002-12-28. 134. “MEMS device for wafer level packaging and method for fabricating the same,” Jin, Jang Seok (KR), KR20020058223 (A)— 2002-07-12. 135. “MEMS packaging using a non-silicon substrate for encapsulation and interconnection,” Heck, John (US), Hayden, Joseph S., III (US) (+2), US2006194361 (A1)—2006-08-31.
35
36
Chapter One 136. “Optical fiber MEMS pressure sensor packaging structure,” Li, Wang Ming (CN), CN2811965 (Y)—2006-08-30. 137. “Low temperature airtightness packaging method for wafer level micro machinery device and photoelectric device,” Wu, Liu Yufei (CN), CN1821052 (A)—2006-08-23. 138. “Heating device for automatic anode linkage of MEMS hightemperature pressure sensor,” Rong, Xie Hui (CN), CN1815705 (A)—2006-08-09. 139. “Packaging of micro devices,” O’Mahony, Conor (IE), Hill, Martin (IE), IE20060046 (A1)—2006-07-26. 140. “Ultra-small profile, low cost chip scale accelerometers of two and three axes based on wafer level packaging,” Liu, Sheng (CN), Chen, Bin (US) (+3), US2006179940 (A1)—200608-17. 141. “Laser assisted chemical etching method for release of microscale and nanoscale devices,” Abraham, Margaret H. (US), Helvajian, Henry (US) (+1), US2006183330 (A1)—200608-17. 142. “Dimesize attitude measurement system in magnetic infrared ray,” Liu, Ye Xiongying (CN), CN1796932 (A)—2006-07-05. 143. “A packaging method for MEMS devices, and MEMS packages produced using the method,” Wang, Zhe (SG), WO2006085825 (A1)—2006-08-17. 144. “Monolithically integrated switchable circuits with MEMS,” Yang, Jeffrey M. (US), Nishimoto, Matt (US) (+3), WO2006083432 (A1)—2006-08-10. 145. “Method and system for packaging MEMS devices with incorporated getter,” Cummings, Manish, Gall, William J. (US), CN1773358 (A)—2006-05-17. 146. “Method and system for packaging a MEMS device,” Miles, Mark W., Sampsell, Jeffrey (US), CN1755473 (A)—2006-04-05. 147. “Apparatus and method for wafer level packaging,” Chen, Jen-Yi (TW), Chiou, Jing-Hung (TW) (+1), TW236111 (B)— 2005-07-11. 148. “Silicon packaging for opto-electronic modules,” Epitaux, Marc (US), WO2006074048 (A2)—2006-07-13. 149. “Integrated MEMS packaging,” Hartzell, John W. (US), Walton, Harry G. (GB) (+1), US2006148137 (A1)—2006-07-06. 150. “System and method for display device with activated desiccant,” Cummings, William J. (US), MXPA05009407 (A)—200603-29.
Introduction to MEMS 151. “Device having patterned spacers for backplates and method of making the same,” Arbuckle, Brian W. (US), MXPA05009402 (A)—2006-03-29. 152. “Injection-molded package for MEMS inertial sensor,” D’Camp, Jon B. (US), Curtis, Harlan L. (US), WO2006068907 (A1)—2006-06-29. 153. “System and method for protecting microelectromechanical system using back-plate with non-flat portion,” Gally, Brian J., Palmateer, Lauren (+1), JP2006119603 (A)—2006-05-11. 154. “Micro-electromechanical varactor with enhanced tuning range,” Chinthakindi, Anil K. (IN), Groves, Robert A. (US) (+3), TW232500 (B)—2005-05-11. 155. “System and method for display device with end-of-life phenomena,” Palmateer, Lauren (US), US2006077524 (A1)—200604-13. 156. “Package for MEMS devices,” D’Camp, Jon B. (US), Curtis, Harlan L. (US), US2006042382 (A1)—2006-03-02. 157. “Micro-fluidic interconnect,” Okandan, Murat (US), Galambos, Paul C. (US) (+2), US7004198 (B1)—2006-02-28. 158. “Semiconductor acceleration sensor system and its manufacturing method,” Kanno, Yoshinori, JP2006003277 (A)—200601-05. 159. “Embedded integrated circuit packaging structure,” Park, Heung-Woo (KR), Song, Jong-Hyeong (KR), US2005275113 (A1)—2005-12-15. 160. “Lead-free bonding systems,” Aggarwal, Ankur (US), Abothu, Isaac R. (US) (+2), US2005274227 (A1)—2005-12-15. 161. “Micro electrical mechanical system (MEMS) tuning using focused ion beams,” Kubena, Randall L. (US), Joyce, Richard J. (US), US2005269901 (A1)—2005-12-08. 162. “Processes for hermetically packaging wafer level microscopic structures,” Cheung, Kin P. (US), US2005189621 (A1)— 2005-09-01. 163. “MEMS device with integral packaging,” Cohn, Michael B. (US), Xu, Ji-Hai (US), US2005168306 (A1)—2005-08-04. 164. “Microelectromechanical systems having trench isolated contacts, and methods for fabricating same,” Partridge, Aaron (US), Lutz, Markus (US) (+1), US2005156260 (A1)—2005-07-21. 165. “Micro connector and non-powered microassembly with micro connector,” Tsui, Kenneth, Geisberger, Aaron (+1), JP2005276816 (A)—2005-10-06.
37
38
Chapter One 166. “Hermetic wafer-level packaging for MEMS devices with low-temperature metallurgy,” Ouellet, Luc (CA), Turcotte, Karine (CA), EP1544164 (A2)—2005-06-22. 167. “Hermetic wafer-level packaging for MEMS devices with low-temperature metallurgy,” Ouellet, Luc (CA), Turcotte, Karine (CA), US2005142685 (A1)—2005-06-30. 168. “Microelectromechanical system and method for determning temperature and moisture profiles within pharmaceutical packaging,” Walker, Dwight S. (US), US2005223827 (A1)— 2005-10-13. 169. “Packaging microelectromechanical structures,” Ma, Qing (US), Rao, Valluri (US) (+3), US2005062120 (A1)—2005-03-24. 170. “Method of making an X-Y axis dual-mass tuning fork gyroscope with vertically integrated electronics and wafer-scale hermetic packaging,” Nasiri, Steven S., Flannery, Anthony Francis, Jr., WO2005043078 (A2)—2005-05-12. 171. “Methods for depositing, releasing and packaging microelectromechanical devices on wafer substrates,” Patel, Satyadev R. (US), Huibers, Andrew G. (US) (+1), US2005048688 (A1)—2005-03-03. 172. “A biological micro spray array dot sample device and method for making same,” Zhao, Jianlong (CN), Xu, Baojian (CN) (+1), CN1629319 (A)—2005-06-22. 173. “Bonding for a micro-electro-mechanical system (MEMS) and MEMS based devices,” Platt, William P. (US), Ford, Carol M. (US), US2004266048 (A1)—2004-12-30. 174. “Micro electro-mechanical variable capacitor,” Chinthakindi, Anil K. (US), US6906905 (B1)—2005-06-14. 175. “Wafer bonding method using reactive foils for massively parallel micro-electromechanical systems packaging,” Snyder, Tanya Jegeris, Yi, Robert H. (+1), JP2005040940 (A)—2005-02-17. 176. “Ultra-miniature accelerometers,” Kenny, Thomas W., Park, Woo-Tae, WO2004092746 (A1)—2004-10-28. 177. “Ultra-miniature accelerometers,” Kenny, Thomas W. (US), Park, Woo-Tae (US), US2004200281 (A1)—2004-10-14. 178. “Magneic switch for use in a system that includes an in-vivo device, and method of use thereof,” Iddan, Gavriel J. (IL), US2004254455 (A1)—2004-12-16. 179. “Magnetic switch for use in a system that includes an in-vivo device, and a method of use thereof,” Iddan, Gavriel J. (IL), WO2004086434 (A2)—2004-10-07.
Introduction to MEMS 180. “Electromechanical system having a controlled atmosphere, and method of fabricating same,” Kronmueller, Silvia (DE), Lutz, Markus (US) (+1), EP1460038 (A2)—2004-09-22. 181. “Optical deflector,” Hara, Koichi, JP2005250307 (A)—200509-15. 182. “Method for fabricating a lid for a wafer level packaged optical MEMS device,” Ehmke, John C. (US), Lopes, Vincent C. (US) (+1), US6856014 (B1)—2005-02-15. 183. “MEMS package,” Brady, Frederick T. (US), US2004099921 (A1)—2004-05-27. 184. “Micro dynamic piezoresistance pressure sensor and manufacturing method thereof,” Wang, Wenxiang (CN), Li, Shuixia (CN) (+1), CN1544901 (A)—2004-11-10. 185. “Processes for hermetically packaging wafer level microscopic structures,” Cheung, Kin P, WO2004037711 (A2)— 2004-05-06. 186. “Processes for hermetically packaging wafer level microscopic structures,” Cheung, Kin P. (US), US2004126953 (A1)— 2004-07-01. 187. “Optical switch and method of producing the same,” Lee, Hyun Kee (KR), Jung, Sung Cheon (KR) (+1), US2004264848 (A1)—2004-12-30. 188. “Method of fabricating an integrated circuit and its precursor assembly,” Ouellet, Luc (CA), Poisson, Jules (CA), EP1405821 (A2)—2004-04-07. 189. “Method of air tight packaging micro computer electric system device using capillary tube method,” Wang, Lichun (CN), Luo, Le (CN) (+1), CN1513751 (A)—2004-07-21. 190. “Latching micro magnetic relay packages and methods of packaging,” Stafford, John (US), Tam, Gordon (US) (+1), US2004027218 (A1)—2004-02-12. 191. “MEMS control chip integration,” Kuo, Shun-Meen, Foerstner, Juergen A (+7), WO2004051744 (A2)—2004-06-17. 192. “Whole wafer MEMS release process,” Dewa, Andrew S. (US), US2004002215 (A1)—2004-01-01. 193. “Encapsulants for protecting MEMS devices during postpackaging release etch,” Peterson, Kenneth A. (US), US6956283 (B1)—2005-10-18. 194. “Method of trimming micro-machined electromechanical sensors (MEMS) devices,” Dwyer, Paul W. (US), US2003196489 (A1)—2003-10-23.
39
40
Chapter One 195. “Methods for depositing, releasing and packaging microelectromechanical devices on wafer substrates,” Patel, Satyadev (US), Huibers, Andrew (US) (+8), WO03105198 (A1)— 2003-12-18. 196. “Microelectromechanical system and method for determining temperature and moisture profiles within pharmaceutical packaging,” Walker, Dwight Sherod (US), WO03107397 (A2)—2003-12-24. 197. “Post-package technology for microelectromechinical system,” Liu, Sheng (CN), Zhang, Honghai (CN) (+1), CN1449990 (A)— 2003-10-22. 198. “On-wafer packaging for rf-MEMS,” Margomenos, Alexandros (US), Herrick, Katherine J. (US) (+2), WO03095357 (A2)—200311-20. 199. “Wafer-level MEMS packaging,” Ouellet, Luc (CA), EP1352877 (A2)—2003-10-15. 200. “Bonding method, bonding device and sealant,” Yuasa, Mitsuhiro, JP2004235465 (A)—2004-08-19. 201. “CMOS compatible microswitches,” Huang, Jung-Tang (TW), Li, Sheng-Hung (TW) (+2), TW565530 (B)—2003-12-11. 202. “Structure and process for packaging rf MEMS and other devices,” Schaper, Leonard W. (US), Malshe, Ajay P. (US) (+1), WO03054927 (A2)—2003-07-03. 203. “Package structure and method for making the same,” Lee, Chenkuo (TW), Yi-Mou, Huang (TW), US2004087043 (A1)— 2004-05-06. 204. “MEMS device sealing packaging method and the fabrication method of metal cap thereof,” Pan, Jeng-Tang (TW), Lin, Kuen-Lung (TW), TW560028 (B)—2003-11-01. 205. “MEMS direct chip attach packaging methodologies and apparatuses for harsh environments,” Okojie, Robert S. (US), US6845664 (B1)—2005-01-25. 206. “Latching micro magnetic relay packages and methods of packaging,” Stafford, John (US), Tam, Gordon (US) (+1), WO03026369 (A1)—2003-03-27. 207. “Electromagnetic actuation optical switch and the fabrication method thereof,” Lu, Hui-Chuan (TW), Lee, Hsin-Li (TW) (+2), TW562951 (B)—2003-11-21. 208. “MEMS wafer level package,” Orcutt, John W. (US), Dewa, Andrew Steven (US) (+1), US2002179986 (A1)—2002-12-05. 209. “A low-cost HDMI-D packaging technique for integrating an efficient reconfigurable antenna array with rf MEMS switches
Introduction to MEMS and a high impedance surface,” Sievenpiper, Daniel F. (US), Schmitz, Adele E. (US) (+3), TW583789 (B)—2004-04-11. 210. “Packaging of MEMS devices using a thermoplastic,” Tourino, Cory G. (US), Rice, Janet L. (US) (+1), US6809412 (B1)—200410-26. 211. “Wafer level MEMS packaging,” Lin, Jong-Kai (US), Lytle, William H. (US) (+5), US2003230798 (A1)—2003-12-18. 212. “Microelectromechanical system device package and packaging method,” Saia, Richard Joseph (US), Durocher, Kevin Matthew (US) (+2), US2002173080 (A1)—2002-11-21. 213. “Surface excited device package including a substrate having a vibration-permitted cavity,” Youl, Min Byoung (KR), Lee, Choon Heung (KR) (+1), US2004164384 (A1)—2004-08-26. 214. “Electrostatically actuated micro-electro-mechanical devices and method of manufacture,” Kudrle, Thomas David (US), Mastrangelo, Carlos Horacio (US) (+6), WO02079853 (A1)— 2002-10-10. 215. “Electrostatically actuated micro-electro-mechanical devices and method of manufacture,” Kudrle, Thomas David (US), Mastrangelo, Carlos Horacio (US) (+6), US2002146200 (A1)— 2002-10-10. 216. “Packaging micromechanical devices,” Low, Yee Leng (US), Ramsey, David Andrew (US), US6603182 (B1)—2003-08-05. 217. “Micromachined fiber optic sensors,” Boyd, Joseph T. (US), Abeysinghe, Don C. (US) (+2), US2002159671 (A1)—200210-31. 218. “Micro-electro-mechanical systems packaging,” West, Glenn S. (SG), Alai, Aijay Babulal (SG) (+1), WO03085732 (A1)—200310-16. 219. “Multilayered microelectronic device package with an integral window,” Peterson, Kenneth A. (US), Watson, Robert D. (US), US6538312 (B1)—2003-03-25. 220. “Photonic component package and method of packaging,” Vaganov, Vladlmin (US), US2003138220 (A1)—2003-07-24. 221. “Method for calibrating a MEMS device,” Gates, John V. (US), Holland, William R. (US) (+2), US2003133644 (A1)— 2003-07-17. 222. “Flex circuit interconnect subassembly and electronic device packaging utilizing same,” Simmons, Richard L. (US), TW548233 (B)—2003-08-21. 223. “Microbar and method of its making,” Kemeny, Zoltan A. (US), US6515346 (B1)—2003-02-04.
41
42
Chapter One 224. “Method of packaging a photonic component and package,” Kohlstadt, Michael (US), Vaganov, Vladmir (US) (+1), US2003113074 (A1)—2003-06-19. 225. “Magnetically packaged optical MEMS device and method for making the same,” Jin, Sungho, Soh, Hyongsok, JP2002236266 (A)—2002-08-23. 226. “Packaging atmosphere and method of packaging a MEMS device,” Henshall, Gordon (GB), Rolt, Stephen (GB), WO0227381 (A2)—2002-04-04. 227. “Method of trimming micro-machined electromechanical sensor (MEMS) devices,” Dwyer, Paul, WO0228766 (A2)— 2002-04-11. 228. “Temporary coatings for protection of microelectronic devices during packaging,” Peterson, Kenneth A. (US), Conley, William R. (US), US6844623 (B1)—2005-01-18. 229. “Wafer level hermetic sealing method,” Cho, Chang-Ho, Shin, Hyung-Jae (+1), JP2002246489 (A)—2002-08-30. 230. “Vacuum package fabrication of integrated circuit components,” Gooch, Roland W. (US), Schimert, Thomas R. (US), US2002000646 (A1)—2002-01-03. 231. “Chip scale surface-mountable packaging method for electronic and MEMS devices,” Kang, Seok-Jin (KR), US2002001873 (A1)—2002-01-03. 232. “Protective fullerene (C60) packaging system for microelectromechanical systems applications,” Olivas, John D. (US), US6791108 (B1)—2004-09-14. 233. “Micro mechanical packaging apparatus,” Degani, Yinon, Dudderar, Thomas D. (+1), JP2002043449 (A)—2002-02-08. 234. “Vacuum package fabrication of microelectromechanical system devices with integrated circuit components,” Gooch, Roland W., Schimert, Thomas R., WO0156921 (A2)—200108-09. 235. “Module with bumps for connection and support,” Pace, Benedict G (US), US6614110 (B1)—2003-09-02. 236. “Guided bullet,” Lipeles, Jay (US), Brosch, R Glenn (US), US2002190155 (A1)—2002-12-19. 237. “Package having cavity for housing MEMS,” Bishop, David John, Gates, John Vanatta (+1), JP2001185635 (A)—2001-07-06. 238. “Improved MEMS wafer-level package,” Oakatto, John W., Dowa, Andrew Steven (+1), JP2001144117 (A)—2001-05-25. 239. “Low-temp MEMS vacuum sealing technique for metals,” Jin, Yufeng (CN), Wu, Guoying (CN) (+1), CN1289659 (A)— 2001-04-04.
Introduction to MEMS 240. “Pre-release plastic packaging of MEMS and IMEMS devices,” Peterson, Kenneth A. (US), Conley, William R. (US), US6379988 (B1)—2002-04-30. 241. “Vacuum package fabrication of microelectromechanical system devices with integrated circuit components,” Gooch, Roland W. (US), US6479320 (B1)—2002-11-12. 242. “Hermetic chip scale packaging means and method including self test,” Bartlett, James L. (US), Wooldridge, James R. (US) (+1), US2003073292 (A1)—2003-04-17. 243. “Cover cap for semiconductor wafer devices,” Karpman, Maurice S. (US), Sengupta, Dipak (US), US6534340 (B1)— 2003-03-18. 244. “Microjoinery methods and devices,” Collins, Scott D. (US), US6393685 (B1)—2002-05-28.
References 1. Madou, M. J. Fundamentals of Microfabrication: The Science of Miniaturization. Boca Raton, FL: CRC Press, 2002. 2. Nguyen, C. “MEMS technology for timing and frequency control.” IEEE Trans. Ultrason. Ferroelect. Freq. Contr. 54:251–270, 2007. 3. Gad-el-Hak, M. The Mems Handbook. Boca Raton, FL: CRC Press, 2002. 4. Hacker, J. B., Mihailovich, R. E., Kim, M., and DeNatale, J. F. “A Ka-band 3-bit rf MEMS true-time-delay network.” IEEE Trans. Microwave Theory Tech. 51: 305–308, 2003. 5. Menz, W., Mohr, J., and Paul, O. Microsystem Technology. Hoboken, NJ: WileyVCH, 2001. 6. Goldsmith, C. L., Yao, Z., Eshelman, S., and Denniston, D. “Performance of low-loss rf MEMS capacitive switches.” IEEE Microwave Wireless Compon. Lett. 8:269–271, 1998. 7. Senturia, S. D. Microsystem Design. New York: Springer, 2000. 8. Rebeiz, G. M. RF MEMS: Theory, Design and Technology. Hoboken, NJ: Wiley, 2003. 9. Anagnostou, D. E., Christodoulou, C. G., Tzeremes, G., Liao, T. S., and Yu, P. K. L. “Fractal antennas with rf-MEMS switches for multiple frequency applications.” In Proceedings of the IEEE APS/URSI International Symposium, Vol. 2, San Antonio, TX, June 2002, pp. 22–25. 10. Yano, M., Yamagishi, F., and Tsuda, T. “Optical MEMS for photonic switchingcompact and stable optical crossconnect switches for simple, fast, and flexible wavelength applications in recent photonic networks.” J. Selected Topics Quantum Elect. 11:383–394, 2005. 11. Anagnostou, D. E., Zheng, G., Chryssomallis, M., Lyke, J. C., Ponchak, G. E., Papapolymerou, J., and Christodoulou, C. G. “Design, fabrication and measurements of a self-similar re-configurable antenna with rf-MEMS switches.” IEEE Trans. Antennas Propagat. 54:422–432, 2006. 12. Liu, A. Q., and Zhang, X. M. “A review of MEMS external-cavity tunable lasers.” J. Micromech. Microeng. 17:R1–R13, 2007. 13. Huff, G. H., and Bernhard, J. T. “Integration of packaged rf MEMS switches with radiation pattern reconfigurable square spiral microstrip antennas.” IEEE Trans. Antennas Propagat. 54:464–469, 2006. 14. Kingsley, N., Anagnostou, D. E., Tentzeris, M., and Papapolymerou, J. “Rf MEMS sequentially reconfigurable Sierpinski antenna on a flexible organic substrate with novel dc-biasing technique.” IEEE/ASME J. Microelectromech. Syst. 16:1185–1192, 2007.
43
44
Chapter One 15. Van Caekenberghe, K., and Sarabandi, K. “A 2-bit Ka-band rf MEMS frequency tunable slot antenna.” IEEE Antennas Wireless Propagat. Lett. 7:179–182, 2008. 16. Nguyen, C. “MEMS technology for timing and frequency control.” IEEE Trans. Ultrason. Ferroelect. Freq. Contr. 54:251–270, 2007. 17. Young, R. M., Adam, J. D., Vale, C. R., Braggins, T. T., Krishnaswamy, S. V., Milton, C. E., Bever, D. W., Chorosinski, L. G., Li-Shu Chen, Crockett, D. E., Freidhoff, C. B., Talisa, S. H., Capelle, E., Tranchini, R., Fende, J. R., Lorthioir, J. M., and Tories, A. R. “Low-loss bandpass rf filter using MEMS capacitance switches to achieve a one-octave tuning range and independently variable bandwidth.” IEEE MTT-S Int. Microwave Symp. Digest 3:1781–1784, 2003. 18. Tan, G. L., Mihailovich, R. E., Hacker, J. B., DeNatale, J. F., and Rebeiz, G. M. “Low-loss 2- and 4-bit TTD MEMS phase shifters based on SP4T switches.” IEEE Trans. Microwave Theory Tech. 51:297–304, 2003. 19. Hacker, J. B., Mihailovich, R. E., Kim, M., and DeNatale, J. F. “A Ka-band 3-bit rf MEMS true-time-delay network.” IEEE Trans. Microwave Theory Tech. 51: 305–308, 2003. 20. Ford, J. E., Goossen, K. W., Walker, J. A., Neilson, D. T., Tennant, D. M., Park, S. Y., and Sulhoff, J. W. “Interference-based micromechanical spectral equalizers.” IEEE J. Selected Topics Quantum Elect. 10:579–587, 2004. 21. Nordquist, C. D., Dyck, C. W., Kraus, G. M., Reines, I. C., Goldsmith, L., Cowan, D., Plut, T.A., Austin, F., IV, Finnegan, P. S., Ballance, M. H., and Sullivan, T. “A dc to 10 GHz 6-bit rf MEMS time delay circuit.” IEEE Microwave Wireless Compon. Lett. 16:305–307, 2006. 22. Perruisseau-Carrier, J., Fritschi, R., Crespo-Valero, P., and Skrivervik, A. K. “Modeling of periodic distributed MEMS application to the design of variable true-time-delay lines.” IEEE Trans. Microwave Theory Tech. 54:383–392, 2006. 23. Kim, C.-H., Park, N., and Kim, Y.-K. “MEMS reflective type variable optical attenuator using off-axis misalignment.” Proc. IEEE/LEOS Int. Conf. Opt. MEMS, Lugano, Switzerland, 2002, pp. 55–56. 24. Lakshminarayanan, B., and Weller, T. M. “Design and modeling of 4-bit slowwave MEMS phase shifters.” IEEE Trans. Microwave Theory Tech. 54:120–127, 2006. 25. Lakshminarayanan, B., and Weller, T. M. “Optimization and implementation of impedance-matched true-time-delay phase shifters on quartz substrate.” IEEE Trans. Microwave Theory Tech. 55:335–342, 2007. 26. Van Caekenberghe, K., and Vaha-Heikkila, T. “An analog rf MEMS slotline true-time-delay phase shifter.” IEEE Trans. Microwave Theory Tech. 56:2151–2159, 2008. 27. Maciel, J. J., Slocum, J. F., Smith, J. K., and Turtle, J. “MEMS electronically steerable antennas for fire control radars.” IEEE Aerosp. Electron. Syst. Mag. Nov. 2007, pp. 17–20. 28. Yeow, T.-W., Law, K. L. E., and Goldenberg, A. “MEMS optical switches.” IEEE Commun. Mag. 39:158–163, 2001. 29. Herrick, K. J., Jerinic, G., Molfino, R. P., Lardizabal, S. M., and Pillans, B. “S-Ku band intelligent amplifier microsystem.” Proc. SPIE 6232, May 2006. 30. Neukermans, A., and Ramaswami, R. “MEMS technology for optical networking.” IEEE Commun. Mag. 39:62–69, 2001. 31. Pranonsatit, S., Holmes, A. S., Robertson, I. D., and Lucyszyn, S. “Single-pole eight-throw rf MEMS rotary switch.” IEEE/ASME J. Microelectromech. Syst. 15:1735–1744, 2006. 32. Lin, L. Y., and Goldstein, E. L. “Opportunities and challenges for MEMS in lightwave communications.” IEEE J. Selected Topics Quantum Elect. 8:163–172, 2002. 33. Vaha-Heikkila, T., Van Caekenberghe, K., Varis, J., Tuovinen, J., and Rebeiz, G. M. “Rf MEMS impedance tuners for 6–24 GHz applications.” Wiley Int. J. RF Microwave Computer-Aided Eng. 17: 265–278, 2007. 34. Syms, R. A., and Moore, D. F. “Optical MEMS for telecoms.” Materials Today 5:26–35, 2002.
Introduction to MEMS 35. Schoebel, J., Buck, T., Reimann, M., Ulm, M., Schneider, M., Jourdain, A., Carchon, G., and Tilmans, H., “Design considerations and technology assessment of phased array antenna systems with rf MEMS for automotive radar applications.” IEEE Trans. Microwave Theory Tech. 53:1968–1975, 2005. 36. Wu, M. C., Solgaard, O., and Ford, J. E. “Optical MEMS for lightwave communication.” J. Lightwave Technol. 24:4433–4454, 2006. 37. Mailloux, R. J. Phased Array Antenna Handbook. New York: Artech House, 2005. 38. Hoffmann. M., and Voges, E. “Bulk silicon micromachining for MEMS in optical communication systems.” J. Micromech. Microeng. 12:349–360, 2002. 39. Jung, C., Lee, M., Li, G. P., and Flaviis, F. D. “Reconfigurable scan-beam singlearm spiral antenna integrated with rf MEMS switches.” IEEE Trans. Antennas Propagat. 54:455–463, 2006. 40. Chang-Hasnain, C. J. “Tunable VCSEL.” J. Selected Topics Quantum Elect. 6: 978–987, 2000. 41. Lijie, J. Z., and Uttamchandani, D. “Integrated self-assembling and holding technique applied to a 3-D MEMS variable optical attenuator.” IEEE J. Microelectromech. Syst. 13:83–90, 2004. 42. Wikipedia. “Microelectromechanical systems:” available at http://en.wikipedia .org/wiki/MEMS, last accessed on April 1, 2008. 43. Yole Development. “World MEMS Markets: The 2006–2012 MEMS Market Database,” 2008. 44. Lau, J. H., Wong, C. P., Lee, N. C., and Lee, R. Electronics Manufacturing with Lead-Free, Halogen-Free, and Adhesive Materials. New York: McGraw-Hill, 2003. 45. Lau, J. H., and Lee, R. Microvias for Low Cost, High Density Interconnects. New York: McGraw-Hill, 2001. 46. Lau, J. H. Low Cost Flip Chip Technologies for DCA, WLCSP, and PBGA Assemblies. New York: McGraw-Hill, 2000. 47. Lau, J. H., and Lee, R. Chip Scale Package Design: Materials, Process, Reliability, and Applications. New York: McGraw-Hill, 1999. 48. Lau, J. H., Wong, C. P., Prince, J., and Nakayama, W. Electronic Packaging: Design, Materials, Process, and Reliability. New York: McGraw-Hill, 1998. 49. Lau, J. H., and Pao, Y. Solder Joint Reliability of BGA, CSP, Flip Chip, and Fine Pitch SMT Assemblies. New York: McGraw-Hill, 1997. 50. Lau, J. H. Flip Chip Technologies. New York: McGraw-Hill, 1996. 51. Lau, J. H. Ball Grid Array Technology. New York: McGraw Hill, 1995. 52. Lau, J. H. Chip on Board Technologies for Multichip Modules. New York: Van Nostrand Reinhold, 1994. 53. Lau, J. H. Handbook of Fine Pitch Surface Mount Technology. New York: Van Nostrand Reinhold, 1994. 54. Lau, J. H. Thermal Stress and Strain in Microelectronics Packaging. New York: Van Nostrand Reinhold, 1993. 55. Lau, J. H. Handbook of Tape Automated Bonding. New York: Van Nostrand Reinhold, 1992. 56. Lau, J. H. Solder Joint Reliability: Theory and Applications. New York: Van Nostrand Reinhold, 1991.
45
This page intentionally left blank
CHAPTER
2
Advanced MEMS Packaging 2.1
Introduction This chapter briefly discusses the state of the art and future trends in advanced integrated circuit (IC) electronics packaging, followed by a discussion of advanced microelectromechanical systems (MEMS) packaging, where 10 different designs of three-dimensional (3D) MEMS packaging will be presented.
2.2 Advanced IC Packaging 3D IC integration with wafer-level packaging (WLP) has been the hottest packaging technology in the past few years and will be the trend in the future. The supply chain of 3D IC integration and WLP includes semiconductor device designers, foundries, packaging and testing houses, electronic design automation (EDA) vendors, processing equipment suppliers, materials suppliers, universities and research institutes, and industry analysts. In this section, the Moore’s law versus more than Moore (MTM) will be discussed briefly first. Next, some of the critical issues of 3D IC integration will be presented. Finally, a couple of enabling technologies (e.g., microbumps and thermal management) for 3D IC integration with WLP will be provided.
2.2.1
Moore’s Law versus More Than Moore (MTM)
In April 1965, Moore published a paper in Electronics with the title, “Cramming More Components onto Integrated Circuits.” Based on a few data points (Figs. 2-1 and 2-2), Moore proposed to put more transistors on an IC by reducing the feature sizes. Further, he suggested that the number of transistors on an IC (for minimum cost) doubles every 24 months. In the past 40+ years, Moore’s observation (law) about silicon integration (i.e., cost, yield, and reliability) has been the most powerful driver for development of the microelectronics industry. This law places emphasis on lithography scaling and integration
47
Chapter Two 16 15 Log2 of the number of components per integrated function
14 13 12 11 10 9 8 7 6 5 4 3 2 1975
1974
1973
1972
1971
1970
1969
1968
1967
1966
1965
1964
1963
1962
1961
1960
1959
1
Year
FIGURE 2-1 The empirical observation made by Moore in 1965 that the number of transistors on an IC for minimum component cost doubles every 24 months. 105 1962 Relative manufacturing cost/component
48
104
1965 103
102
1970
10
1 1
10
102
103
104
105
Number of components per integrated circuit
FIGURE 2-2 Moore’s observation about silicon integration (i.e., cost, yield, and reliability) has fueled the worldwide technology revolution: (1) IC miniaturization down to the nanoscale and (2) SoC-based system integration.
Advanced MEMS Packaging
MEMS ASIC
Seal ring
FIGURE 2-3 The accelerometer MEMS device is integrated into the ASIC chip by Analog Devices. On the other hand, the same functions can be achieved by stacking the MEMS device on the ASIC chip, resulting in 3D MEMS packaging.
[in two dimensions (2D)] of all functions on a single chip, perhaps through system-on-chip (SoC) capabilities. Today, 32-nm ICs are in volume production, and production of 28-nm ICs is planned to begin in the second half of 2010. In the meantime, 22-nm technology has been working/performing very well in research institutions and laboratories. On the other hand, integration of all these functions can be achieved through system-in-package (SiP) or, ultimately, 3D IC integration and WLP, which is called more than Moore (MTM).1–54 Figure 2-3 shows an example of Moore’s law (2D) versus MTM (3D). It can be seen from the left side of the figure that the accelerometer MEMS device is integrated into the ASIC chip by Analog Devices. On the other hand, the same functions can be achieved by stacking the MEMS device on the ASIC chip,52–54 resulting in 3D MEMS packaging (or 3D MEMS SiP or 3D MEMS WLP), which is the focus of this book. It should be pointed out that MTM is much more than just SiP. Based on the silicon-platform technology, anything that involves the integration of electronics, photonics, mechanics, chemistry, heat, magnetics, biology, etc., for functionality and system performance when interacting with people and the environment can be called MTM. One of the reasons why MEMS is called MTM is because the microelectronic ICs are thought of as the “brains” of a system, and MEMS augments this decision-making capability with “eyes” and “arms” to allow microsystems to sense and control the environment.
2.2.2
3D IC Integration with WLP
The Holy Grail of 3D IC integration (heterogeneous integration) is shown in Fig. 2-4, where all the chips [e.g., microdisplay, MEMS, memory, microprocessor, multiple outputs dc-dc converter, digital signal processor, microbattery, and analog-to-digital (A/D) mixed signal]
49
50
Chapter Two
DSP B A
Memory Display B
DSP
OPTO
Display
Processor Memory
MEMS
Long wiring (from A to B) in 2D SoC
OPTO
MEMS TSV
A
Micro bumps
Processor
Short wiring (from A to B) in 3D IC integration with TSV and microbumps
FIGURE 2-4 The Holy Grail of 3D IC integration (heterogeneous integration) with TSV, which provides shorter wiring than 2D SoC.
are stacking in three dimensions. Just as with many other new technologies, 3D IC integration still faces many critical issues. In the development of 3D IC integration, the following must be noted and understood:1–24 • Design guidelines and software are not available. • Test methods and equipment are lacking. • Known good dies (KGDs) are required. • Through-silicon vias (TSVs) with redistribution layers (RDLs) usually are required. • Microbumps usually are required. • Equipment accuracy is necessary for alignments. • Fast chips must be mixed with slow chips. • Large chips must be mixed with small chips. • Wafer thinning and thin-wafer handling during processing are necessary. • Thermal issues: • The heat flux generated by stacked multifunctional chips in miniature packages is extremely high. • 3D circuits increase total power generated per unit surface area. • Chips in the 3D stack may be overheated if proper and adequate cooling is not provided. • The space between the 3D stack may be too small for cooling channels (i.e., no gap for fluid flow).
Advanced MEMS Packaging • Thin chips may create extreme conditions for on-chip hot spots. • 3D IC stacking inspection methodology is needed. • 3D IC stacking expertise is lacking. • 3D IC stacking infrastructure is lacking. • 3D IC stacking standards are lacking. In the past few years, some of these critical issues have been studied by a number of experts. Their results have already been disclosed in diverse journals or, more specifically, in the proceedings of many conferences, symposia, and workshops whose primary emphases have been on electrical packaging and interconnection. Consequently, there is no single source of information devoted to the state of the art of 3D IC integration with WLP technology. This section briefly mentions only microbumps and thermal management of 3D IC integration. The other important enabling technology (e.g., TSV; wafer thinning and thin-wafer handling; thin-wafer strengthening; wafer dicing; underfilling; lead-free soldering; low-temperature bonding; chip-to-chip (C2C), chip-to-wafer (C2W), and wafer-to-wafer (W2W) bonding; and in situ stress measurement for MEMS applications) will be discussed throughout the remaining chapters of this book. Figure 2-5 shows a generic 3D IC packaging roadmap provided by IBM.1 It can be seen from the “Chip-to-chip/chip-to-wafer” line that microbumps are used for connecting the high-performance chips and the TSV silicon carrier (interposer) and the 3D TSV memory-chip stack. Figure 2-6 shows Intel’s proposed roadmap of package-architecture
Wafer to wafer
3D Si integration
Device layer 2 Vertical interconnect Device layer 2
Silicon
Chip to chip/chip to wafer Performance
Silicon carrier Chip 1 Chip 2
TSV for interposer
3D chip stack
Substrate
TSV for 3D chip stacking
Chip to package Caramic and organic packages Evolutionary improvements Printed circuit card 2000
2005
2010 Time
FIGURE 2-5 IBM’s generic 3D IC packaging roadmap.
2015
51
52
Chapter Two 3D Stackeddie MCP Memory CPU
Substrateembeddeddie MCP 2D Planar MCP
BW > 1 TB/s
CPU Memory
BW = 200 GB/s–1 TB/s CPU
Memory
Off-pkg BW = 100–200 GB/s CPU
Memory
BW < 100 GB/s
FIGURE 2-6 Intel’s proposed roadmap of package-architecture transitions to address the memory-bandwidth challenge.
transitions to address the memory-bandwidth challenge.14 It can be seen that 3D stacked-die multiple-chip packaging is needed to meet the performance requirements and that microbumps are used to connect the memory chip to the central processor unit (CPU).
2.2.3
Low-Cost Solder Microbumps for 3D IC SiP
The material used for connecting high-pin-count, small-pad, and finepitch chips can be either high-cost metal bumps (e.g., copper and gold) or low-cost solder bumps (e.g., tin). In this section, only low-cost solder microbumps will be discussed. Figure 2-7 is a schematic of the 3D stacking of a memory chip and an Si carrier chip (could be the CPU) with TSV.21 There are more than 4000 solder microbumps between them, and their distribution is shown in Fig. 2-8. The functional bumps are concentrated in a
Si chip Solder microbumps
TSV
UBM pad 25 Si carrier μm
Ordinary solder bumps
FIGURE 2-7 Schematic of the 3D stacking of a memory chip and an Si carrier (could be a CPU) at 25 μm pitch.
Advanced MEMS Packaging
All the others are dummy bumps/UBM pads for stability assembly
Bumps/UBM pads for interconnection
FIGURE 2-8 Distribution of solder microbumps/under-bump-metallurgy (UBM) pads on an Si chip/Si carrier (not in scale).
very narrow strip with very fine pitches (≤25 μm) and small pads (≤15 μm), and the dummy bumps (to provide support during assembly and to absorb the stresses and strains of thermal-expansion mismatch between the Si chip and the copper-filled TSV chip) are around the edges. Figure 2-9 shows a schematic of the cross section of a solder microbump on an Si chip. It can be seen that it consists of the metal pad and a Ti (or Ta) adhesion layer, Cu seed layer, plated Cu layer, plated Sn layer, and passivation layer. Figure 2-10 shows a schematic of the cross section of an electroless Ni and immersion Au (ENIG) under-bump metallurgy (UBM) pad. It can be seen that it consists of the Al pad, Ni layer, Au layer, and two passivation layers.
a. Bump height
b
b. Bump width c. Ti adhesion
g
a
d. Cu seed layer e. Cu f. Sn g. Passivation: SiO2
f e d
c Metal pad Si chip
FIGURE 2-9 Schematic of the cross section of a solder microbump on an Si chip.
53
54
Chapter Two FIGURE 2-10 Schematic of the cross section of the electroless Ni and immersion Au (ENIG) UBM pad.
d
e
c b a f Si carrier
a. Passivation 1 (SiO2) b. Passivation 2 (SiO2) c. Al pad (daisy chain) d. Electroless Ni e. Immersion Au f. Al pad opening
Figure 2-11 shows scanning electron microscope (SEM) images of the electroplated Cu-Sn solder microbumps on an Si chip, and Fig. 2-12 shows the Cu-Sn solder microbumps on an Si chip after reflow at 265°C. Figure 2-13 shows a focused-ion-beam (FIB) image of the Cu-Sn solder microbumps on an Si chip. It can be seen that nice and smooth Cu-Sn solder microbumps on a 25-μm pitch and 15-μm pad have been achieved.
Plated Sn at 25-μm pitch
10 μm
FIGURE 2-11 SEM image of the electroplated Cu-Sn solder microbumps on an Si chip.
Advanced MEMS Packaging Reflowed Sn at 25-μm pitch
10 μm
FIGURE 2-12 SEM image of the Cu-Sn solder microbumps on an Si chip after reflow at 265°C.
Cu6Sn3
Cu3Sn
Sn
Cu
FIGURE 2-13 FIB image of the Cu-Sn solder microbumps on an Si chip.
55
56
Chapter Two Electroless Ni & lmmersion Au at 25-μm pitch
FIGURE 2-14 SEM image of ENIG UBM on an Si carrier.
Just as with ordinary solder bumps, there are two layers of intermetallic compounds (IMCs), the Cu3Sn and Cu6Sn5. Figures 2-14 and 2-15 show, respectively, SEM and FIB images of the ENIG UBM on an Si carrier. It can be seen that the Ni layer is about 4 μm thick and that there is no cracking around the edges of
FIGURE 2-15 FIB image of ENIG UBM on an Si carrier.
4 μm
Au Ni
Passivation
Advanced MEMS Packaging
Chip with solder bumps Cu Sn Ni
Chip with UBMs μm
μm
FIGURE 2-16 SEM images of the assembly cross section of an Si chip and Si carrier (15 μm pitch and 8 µm pad).
the passivations. A similar UBM has been made for a 15-μm pitch and 8-μm pad. In this case, the Ni layer is about 2 μm thick.22 Figure 2-16 shows the assembly of an Si chip and Si carrier with 15-μm pitch and 8-μm pad Cu-Sn solder microbumps. It can be seen from the cross section that the micro solder joints between these chips can be assembled properly and that the standoff is about 12 μm, which is preferred for 3D IC stacking and SiP. The effective thermal expansion coefficient of the Cu-filled TSV Si carrier (~10 × 10–6/°C) is larger than that (~2.5 × 10–6/°C) of the Si chip, and therefore, underfill may be necessary to ensure the reliability of the micro solder joint. Figure 2-17 shows an optical photograph of
Si chip
Si chip Underfill
Underfill in the assembly gap Si carrier Si carrier Si chip Si chip Underfill and microbumps in the assembly gap
Underfill
FIGURE 2-17 Optical photograph of a cross section of the underfill between an Si chip and Si carrier.
57
58
Chapter Two a cross section of underfill between these two chips. For results of shearing and thermal cycling tests for these micro solder joint assemblies, please see refs. 21 and 22, which demonstrate that these solder microbumps are adequate for most operating conditions.
2.2.4 Thermal Management of 3D IC SiP with TSV As mentioned earlier, thermal management is one of the critical issues of 3D IC integration. Thus low-cost and effective thermal management design guidelines and solutions are desperately needed for widespread use of 3D IC integration. Based on the theory of heat transfer, this section examines the thermal performance of 3D stacking of up to eight copper-filled TSV chips. The results are plotted in useful design charts for engineering practice convenience, and design guidelines are also provided.20 In order to have a miniature product with low-profit and smallform-factor components, the chip thickness in a 3D stacked component must be very thin (e.g., 50 μm or less). Unfortunately, chip temperature and the hot-spot temperature in a chip increase with reductions in chip thickness, which poses significant thermal management challenges. This section also presents heat-transfer analysis of a (5 × 5 mm) chip with different thicknesses (from 10 to 200 μm) subjected to various heat sources. In addition, the thermal coupling effects of a (5 × 5 × 0.05 mm) chip subjected to heat sources at various locations are presented. Again, useful design charts and design guidelines relating the important parameters are provided. Even with the most effective software and advanced high-speed hardware, it is impossible to model all the TSVs in a 3D IC integration SiP. Therefore, this section develops empirical equations for the equivalent thermal conductivity of a copper-filled TSV chip with various TSV diameters, pitches, and aspect ratios through detailed 3D heat-transfer Computational Fluid Dynamic (CFD) analysis. These equations then are used (for each TSV chip as a lumped block) to perform all the simulations reported herein.
Equivalent Thermal Conductive of TSV Chips Figure 2-18 is a schematic of a 3D IC integration of eight copperfilled TSV chips. The top-layer chip does not (and does not need to) have a TSV. These chips are connected through microbumps, and the bottom TSV chip is also connected to the organic printed circuit board (PCB) by ordinary flip-chip solder bumps. Owing to the large thermal expansion mismatch between the silicon chip and the organic PCB, underfill is needed to cement the bottom chip (and the stack) to the PCB so that the solder joints are reliable. Underfill may not be necessary between all the TSV chips. As mentioned earlier, this section determines the equivalent thermal conductivity of the copper-filled TSV chips through detailed 3D
Advanced MEMS Packaging Copper-filled TSV (many)
TSV chip
TSV
z
y x
Micro bump
Chip q T
Solder bump
Adiabatic
Δz PCB
Underfill
Adiabatic
Δz q = –keq,z dT = k eq,z ΔT ⇒ k eq,z = q Δz dz ΔT ΔT Δx q = –keq,x dT = k eq,x ⇒ k eq,x = q dx Δx ΔT keq,y = keq,x
Isotherm (T1 = 25°C)
T q Adiabatic
Δx
FIGURE 2-18 Schematic of a 3D IC integration of eight copper-filled TSV chips along with the equivalent thermal conductive model and boundary conditions.
CFD analysis. One of the TSV chip is shown schematically in the upper right-hand corner of Fig. 2-18. It can be seen that unlike the thermal conductivity of an ordinary silicon chip [150 W/(m · °C)], which is isotropic, the thermal conductivity of a copper-filled TSV silicon chip is anisotropic; that is, the thermal conductivity in the xy-planar directions (keq,x = keq,y) is not equal to that in z-normal direction (keq,z). [The thermal conductivity of copper is 390 W/(m · °C).] The approaches for extracting keq,x = keq,y and keq,z are shown, respectively, in the center and bottom right-hand side of Fig. 2-18. First, construct the geometry of the copper-filled TSV chip with various diameters, pitches, and aspect ratios. Then input the thermal material properties [the thermal conductivity of silicon is 150 W/(m · °C) and that of copper is 390 W/(m · °C)]. Finally, apply the kinetic and kinematic boundary conditions, and calculate the temperature distributions. The equivalent thermal conductivity can be obtained with the equations shown in the lower left-hand corner of Fig. 2-18. For example, to extract the equivalent thermal conductivity in the z direction, the geometry of the TSV chip is constructed, then a uniform heat flux q is imposed on the top surface of the TSV chip, and the bottom surface is set as an isotherm boundary (i.e., 25°C), whereas the four surrounding boundaries are set as adiabatic boundaries. By using the Flowtherm software, the average temperature on the top surface of the TSV chip can be calculated, and consequently, keq,z can be obtained using the first equation in the figure.
59
Chapter Two 260 Equivalent conductivity, W/(m·K)
250
Pitch = 0.2 mm, Keq,z Pitch = 0.3 mm, Keq,z Pitch = 0.5 mm, Keq,z
240
Pitch = 0.25 mm, Keq,z Pitch = 0.4 mm, Keq,z Pitch = 0.6 mm, Keq,z
230 Keq, z
220 Pitch: 0.3 mm – correlation
210
D1
D1
200 0.3 mm
190
P
180
D2
D2
170 160 150 140 2
4
6
8
10
Aspect ratio, A keq,z = 150 + 188D 2P –2; D = (D1 + D2)/2; A = thickness/D
FIGURE 2-19 The equivalent thermal conductivity (in the vertical direction) for a copper-filled TSV chip with various diameters, pitches, and aspect ratios.
Figures 2-19 and 2-20, respectively, show the equivalent thermal conductivity for keq,z and keq,x = keq,y of a copper-filled TSV chip with various diameters, pitches, and aspect ratios. It can be seen that (1) the equivalent thermal conductivity in all directions of the TSV chip is 260 250 Equivalent conductivity, W/(m·K)
60
Pitch = 0.2 mm, Keq,x,y Pitch = 0.3 mm, Keq,x,y Pitch = 0.5 mm, Keq,x,y
240
Pitch = 0.25 mm, Keq,x,y Pitch = 0.4 mm, Keq,x,y Pitch = 0.6 mm, Keq,x,y
230 220 210 200
Pitch: 0.30 mm – correlation
190
Keq,x,y
D1 0.3 mm
D1 P
180
D2
170
D2
160 150 140 2
4
6 Aspect ratio, A
8
10
keq,x = keq,y = 150 + 105D 2P –2; D = (D1 + D2)/2; A = thickness/D
FIGURE 2-20 The equivalent thermal conductivity (in the horizontal direction) for a copper-filled TSV chip with various diameters, pitches, and aspect ratios.
Advanced MEMS Packaging larger than that of a pure silicon chip, (2) the equivalent thermal conductivity in all directions is larger for smaller pitches of the TSV chip, and (3) the equivalent thermal conductivity in all directions is larger for larger diameters of the TSV chip. For engineering convenience, the results in Figs. 2-19 and 2-20 have been curve-fitted into the following empirical equations for equivalent thermal conductivity: keq,z = 150 + 188D2P–2 keq,x = keq,y = 150 + 105D2P–2 where P is the pitch, D = (D1 + D2)/2 is the diameter, and D1 and D2 are the diameters of a tapered TSV chip. The accuracy of these equations has been demonstrated by showing the correlation between the empirical equations (for the case of P = 0.3 mm) with the detailed 3D CFD analyses, as shown in Figs. 2-19 and 2-20. Consequently, these empirical equations will be used for TSV chips as a lumped block without any vias for analysis of the 3D SiP. Table 2-1 shows the material properties for the simulations.
Thermal Performance of 3D Stacked TSV Chips with a Uniform Heat Source Figure 2-21 shows the maximum junction temperature of a stackedchip (varying with the number of the chips) package. In these simulations, all the chips have the same size (5 × 5 × 0.05 mm), and there are 225 (15 × 15) copper-filled TSVs with a 0.2-mm pitch on each chip. The power dissipated by each chip is 0.2 W, and it is assumed that the power is uniformly distributed on each chip. The ambient temperature is 25°C. It can be seen from the figure that the maximum junction temperature increases linearly with the number of the chips stacked. In addition, it can be seen that if the maximum allowable junction temperature is 85°C, then the maximum number of chips that can be stacked together is seven under the present conditions. Figure 2-22 shows the maximum junction temperature at each layer of the TSV chip stack. It can be seen that the maximum junction
Chip
TSV
Bumps
Underfill
PCB
Material
Si (TSV)
Cu
SnAg
Polymer
FR4
K [W/(m · °C)]
Empirical equation
390
57
0.5
// 0.8 ⊥ 0.3
Dimension (mm)
5×5
Ø = 0.05
Ø = 0.20 Height = 0.15
5×5× 0.15
76 × 114 × 1.6
Power (W)
0.2 W
NA
NA
NA
NA
TABLE 2-1
Material Properties and Dimensions of 3D IC Integration
61
62
Chapter Two
Max. junction temperature, Tj (°C)
95 85
Tj = 85°C
Uniform 75 heat source over the 65 whole TSV chip 55
TSV chip
45
Chip thickness = 50 μm Chip power = 0.2 W/chip Heat source area = 5 × 5 mm
35 25
0
2
4
6
8
10
Number of stacked TSV chips
Max. Temperature, °C
FIGURE 2-21 Maximum junction temperature of the eight stacked chips.
90
85
Chip thickness = 50 μm Chip power = 0.2 W/chip Heat source area = 5 × 5 mm
0
2
4
6
8
Layer of TSV chip (from the bottom)
FIGURE 2-22 Maximum junction temperature at each layer of the TSV chip stack.
temperature difference between each layer of the stack is negligible. This means that the temperature distribution for the different layer of chips is uniform because we assumed that the power dissipation is uniformly distributed in each chip. Figure 2-23 shows the variation in thermal resistance of the SiP with the number of the TSV chips stacked. The materials, geometry, boundary conditions, and assumptions are the same as those in Fig. 2-21. It can be seen that the thermal resistance of the stacked SiP decreases as the number of chip in the stack increases.
Advanced MEMS Packaging
Thermal resistance, Rja (°C/W)
45
Uniform heat source over the whole TSV chip
44 43 42 41
TSV chip
40 39 38
Chip thickness = 50 μm Chip power = 0.2 W/chip Heat source area = 5 × 5 mm
37 46 35
0
2
4 6 Number of stacked TSV chips
8
10
FIGURE 2-23 Variation in thermal resistance of the SiP with the number of TSV stacked chips.
Thermal Performance of 3D Stacked TSV Chips with a Nonuniform Heat Source The results presented in Figures 2-21, 2-22, and 2-23 are based on the assumption that the power is dissipated uniformly over the whole chip. However, in most applications, the power dissipated by each chip is basically nonuniform, and as such, it will induce quite different thermal behaviors of the 3D IC SiP with TSV chips. In addition, it is well known that ordinary silicon chips normally have large parallel conduction of heat (parallel to the chip surface) owing to the large thermal conductivity of the Si material. However, for 3D IC chip stacking, in order to have a low profile, the chip thickness of each layer of the 3D SiP must be ground down to 50 μm and less. Thus the parallel spreading effect is suppressed by the very thin chip, and the hot spot will be very intense. Compounding this with the nonuniform heat source, the hot spot becomes a challenge in 3D IC integration SiP. Figures 2-24, 2-25, and 2-26 show the thermal performance of a 3D integration of two copper-filled TSV chips stacking in an SiP, where a single copper-filled TSV chip is also included. All the chips are 5 × 5 mm, and their thicknesses vary from 10 to 200 μm. Each chip’s center is subjected to a distinct heat source (0.2 W) in a tiny area (0.2 × 02 mm). It can be seen from Figs. 2-24 and 2-25 that (for both one- and two-chip stacks) (1) for a nonuniform heat source, the effect of chip thickness on the thermal performance of 3D IC integrations is very important, (2) this thickness effect is even more significant in the application range (≤50 μm) of 3D IC integrations, and (3) the maximum junction temperature and thermal resistance decrease as chip thickness increases.
63
Chapter Two
Max. Junction temperature Tj (°C)
95 85 75
Two TSV chips
Heat source
65 One TSV chip
55
Chip
45 Chip power = 0.2 W/chip Chip heat source area = 0.2 × 0.2 mm
35 25
0
50
100 TSV chip thickness, μm
150
200
FIGURE 2-24 Maximum junction temperature of a 3D integration of two Cu-filled TSV chips.
250 Thermal resistance, Rja (°C/W)
64
200 Two TSV chips
150
Heat source One TSV chip
100
Chip
50
0
Chip power = 0.2 W/chip Chip heat source area = 0.2 × 0.2 mm 0
50
100 TSV chip thickness, μm
150
200
FIGURE 2-25 Thermal resistance of a 3D integration of two Cu-filled TSV chips.
Figure 2-26 shows the temperature maps on the chip for various chip thicknesses. It can be seen that the heat on the chip surface is well dissipated for typical chip thicknesses of 100 to 200 μm subjected to a generated power of 0.2 W. For the 200-μm-thick chip, the temperature distribution is almost uniform and equal to 35°C. However, the hot-spot temperature on the chip increases to 69°C (0.2-W power) if the chip thickness is reduced to 10 μm, and the hot-spot area is clearly shown.
Advanced MEMS Packaging t = 10 μm
t = 25 μm
t = 100 μm
t = 50 μm
t = 200 μm Temperature (°C) 68.9
49.5
Chip power: 0.2 W/chip Chip heat source area: 0.2 × 0.2 mm
30
FIGURE 2-26 Temperature maps on the chip for various chip thicknesses (hot spots).
In addition to one heat source per chip (5 × 5 mm), Figs. 2-27 and 2-28 show the effect of two heat sources at a distance apart (gap) on the thermal performance of 3D IC integrations of copper-filled TSV chips. There are two distinct heat sources (each with 0.1 W and on 0.2 × 0.2 mm area) on each chip (5 × 5 × 0.05 mm). It can be seen from the
Max. junction temperature, Tj (°C)
60
a
Chip power = 0.2 W/chip b
55
50
Heat source area = 0.2 × 0.2 mm
Two TSV chips
45 One TSV chip
40
35
0
0.2
0.4 0.6 Gap between heat sources, b/a
0.8
FIGURE 2-27 Maximum junction temperature of a 3D integration of two Cu-filled TSV chips subjected to two distinct heat sources.
1
65
Chapter Two 110 Thermal resistance, Rja (°C/W)
66
a
100
b
Chip power = 0.2 W/chip Heat source area = 0.2 × 0.2 mm
90 80
One TSV chip
70 Two TSV chips
60 50
0
0.2
0.4
0.6
0.8
1
Gap between heat sources, b/a
FIGURE 2-28 Thermal resistance of a 3D integration of two Cu-filled TSV chips subjected to two distinct heat sources.
figures that (1) the larger the gap (b/a ≤ 0.7) between the two heat sources, the better is the thermal performance (i.e., lower maximum junction temperature and thermal resistance), and (2) when the gap between the two heat sources is larger than 0.7 (i.e., the heat sources are too close to the edge of the chip), the thermal performance is weaker. This is due to suppressible spreading effects near the edges of the chips. In addition to the case of overlapping heat sources discussed in the preceding paragraph, finally, Figs. 2-29 and 2-30 show the orientation effect (staggered heat sources) of two stacked chips, each with two heat sources at a certain distance apart, on the thermal performance of a 3D SiP. It can be seen that (1) similar to case of overlapping heat sources, the larger the gap (b/a ≤ 0.7) between those two pairs of staggered heat sources, the lower are the maximum junction temperature and thermal resistance, (2) when the gap between the two pairs of staggered heat sources is larger than 0.7 (i.e., the heat sources are too close to the edge of the chip), the thermal performance is weaker, and (3) the maximum junction temperature and thermal resistance of the 3D SiP with two TSV chips subjected to two pairs of staggered heat sources are lower than those with two pairs of overlapping heat sources. This is so because the staggered heat sources avoid the superimposition of heat sources and thus lead to better thermal performance. This result is very useful for the design and layout 3D SiP because it permits relocation of the heat sources and/or rotation of the chip.
Advanced MEMS Packaging
Max. Junction temperature, Tj (°C)
55
a
Chip power = 0.2 W/chip Heat source area = 0.2 × 0.2 mm
a
54 b
53
b
52 51
Overlapped sources
50
2 TSV chips with over lapped heat sources
Staggered sources
49 48
2 TSV chips with staggered heat sources
47 46 45
0
0.2
0.4 0.6 Gap between heat sources, b/a
0.8
1
FIGURE 2-29 Maximum junction temperature of a 3D integration of two Cu-filled TSV chips subjected to two distinct staggered heat sources.
75
Thermal resistance, Rja (°C/W)
a b
70
65
Chip power = 0.2 W/chip Heat source area = 0.2 × 0.2 mm
a b
Overlapped sources
2 TSV chips with overlapped heat sources
Staggered sources
60 2 TSV chips with staggered heat sources
55
50
0
0.2
0.4
0.6
0.8
1
Gap between heat sources, b/a
FIGURE 2-30 Thermal resistance of a 3D integration of two Cu-filled TSV chips subjected to two distinct staggered heat sources.
2.3 Advanced MEMS Packaging Advanced MEMS packaging usually involves at least three wafers, namely, the MEMS device wafer, the ASIC wafer, and the cavity-cap wafer. This section examines the design and processing of 10 different configurations of 3D MEMS packaging.53 These packages are supposed to yield very low-cost, high-performance packaging with a small footprint.
67
68
Chapter Two Solder bump with TSV substrate
MEMS wafer
Note: Cases 1 to 6 should have the cap without TSV
Solder bump flip-chip without TSV Wire bond
ASIC wafer
5
6
2
3
4 1
With TSV
8
9
7
Without TSV
Note: Cases 7 to 9 should have the ASIC without TSV
Cap wafer TSV in cap
FIGURE 2-31 Nine different designs of 3D MEMS packaging for the MEMS wafer, ASIC wafer, and cavity-cap wafer.
2.3.1
3D MEMS WLP: Designs and Materials
Figure 2-31 shows nine different combinations (designs) of 3D MEMS packaging from the MEMS wafer (with either wire-bonding pads, solder-bumped TSV substrate, or solder-bumped flip-chip without TSV), the ASIC wafer (with or without TSV), and the cavity-cap wafer (with or without TSV).53 Case 1: The MEMS device is die attached and then wire bonded on the ASIC chip or wafer. The cavity-cap chip/wafer is attached to the ASIC chip/wafer with a sealing ring, as shown in Fig. 2-32. Cavity-cap
Wire bondIng
Sealing ring
MEMS device
ASIC chip Signal lines go through beneath sealing ring to wire-bonding pad on the chip periphery
Circuitry
MEMS chip (substrate)
Bonding pad on a substrate or PCB
FIGURE 2-32 All wire-bonding 3D MEMS packaging with lateral electrical feedthrough.
Advanced MEMS Packaging MEMS device and substrate with TSV
Cavity-cap Sealing ring
Wire bonding
ASIC chip Signal lines go through beneath sealing ring to wire-bonding pad on the chip periphery
Circuitry
Tiny solder bumps
Bonding pad on a substrate or PCB
FIGURE 2-33 Solder-bumped MEMS device with TSV substrate on an ASIC chip with lateral electrical feed-through.
The signal lines go through beneath the sealing ring to the wirebonding pad on the ASIC chip periphery. Another set of wirebonding pads connects the MEMS/ASIC 3D stack to either a substrate in a package or on a PCB. Case 2: The micro-solder-bumped MEMS device with a TSV substrate is first attached to the ASIC, as shown in Fig. 2-33. The rest is the same as in case 1. Case 3: The solder-bumped flip-chip MEMS device is first attached on the ASIC, as shown in Fig. 2-34. The rest is the same as in case 1. Case 4: The MEMS device is die attached and wire bonded on the ASIC chip with TSV and ordinary solder bumps, as shown in Fig. 2-35. A cavity cap is attached on the ASIC with a sealing ring. The MEMS/ASIC 3D stack is then attached (solder reflowed) to a substrate in a package or on a PCB.
MEMS device and substrate with solder bumps Cavity-cap Sealing ring Wire bonding
ASIC chip Signal lines go through beneath sealing ring to wire-bonding pad on the chip periphery
Circuitry Solder bumps
Bonding pad on a substrate or PCB
FIGURE 2-34 Solder-bumped flip-chip MEMS device on an ASIC chip with lateral electrical feed-through.
69
70
Chapter Two Wire bonding Sealing ring
Cavity-cap
MEMS device
ASIC chip
Ordinary solder bumps MEMS chip (substrate)
Through-silicon via (TSV)
FIGURE 2.35 MEMS device wire bonded on an ASIC chip with vertical electrical feed-through TSV.
MEMS substrate with TSV Cavity-cap Sealing ring
MEMS device
ASIC chip
Ordinary solder bumps Tiny solder bumps
Through-silicon via (TSV)
FIGURE 2.36 TSV MEMS device solder bonded on an ASIC chip with vertical electrical feed-through TSV.
Case 5: The micro-solder-bumped MEMS device with a TSV substrate is first attached to the ASIC chip with TSV and ordinary solder bumps, as shown in Fig. 2-36. The rest is the same as in case 4. Case 6: The solder-bumped MEMS device is first attached to the TSV ASIC with ordinary solder bumps, as shown in Fig. 2-37. The rest is the same as in case 5. Case 7: The MEMS device is die attached and then wire bonded on the ASIC. The cavity cap with TSV and ordinary solder bumps is attached to the ASIC with a sealing ring, as shown in Fig. 2-38. Then the whole 3D carrier is attached (solder reflowed) to a substrate in a package or on a PCB. Case 8: The micro-solder-bumped MEMS device with TSV substrate is first attached to the ASIC as shown in Fig. 2-39. The rest is the same as in case 7.
Advanced MEMS Packaging MEMS substrate with solder bumps Cavity-cap Solder bumps
Sealing ring
ASIC chip
Ordinary solder bumps
Through-silicon via (TSV)
MEMS device
FIGURE 2-37 Solder-bumped MEMS device flip-chip on an ASIC chip with vertical electrical feed-through TSV. Ordinary solder bumps Cavity-cap Through-silicon via (TSV)
Wire bonding Sealing ring
MEMS device
ASIC chip MEMS chip (substrate)
FIGURE 2-38 MEMS device wire bonded on an ASIC chip (vertical electrical feed-through TSV is in the package cap). Ordinary solder bumps Cavity-cap Sealing ring Through-silicon via (TSV)
MEMS device
ASIC chip MEMS substrate with TSV
Tiny solder bumps
FIGURE 2-39 TSV MEMS device solder bonded on an ASIC chip (vertical electrical feed-through TSV is in the package cap).
Case 9: The solder-bumped MEMS device is first attached to the ASIC as shown in Fig. 2-40. The rest is the same as in case 7. Case 10: The MEMS device is attached to the ordinary solderbumped TSV ASIC with a sealing ring, as shown in Fig. 2-41. Then the whole 3D stack is attached (solder reflowed) to a substrate in a package or on a PCB.
71
72
Chapter Two Ordinary solder bumps Cavity-cap Sealing ring Through-silicon via (TSV) ASIC chip MEMS device
Solder bumps
MEMS substrate with solder bumps
FIGURE 2-40 Solder-bumped MEMS device flip-chip on an ASIC chip (vertical electrical feed-through TSV is in the package cap). MEMS substrate
Sealing ring
ASIC chip
Ordinary solder bumps MEMS device
Through-silicon via (TSV)
FIGURE 2-41 MEMS device is bonded (with a sealing ring) on an ASIC chip with vertical electrical feed-through TSV.
2.3.2
3D MEMS WLP: Processes
There are many different processes to assemble these 10 MEMS SiPs. For example, the assembly process shown in Fig. 2-42 can be applied to cases 1 through 3; Fig. 2-43, to cases 4 to 6; and Fig. 2-44, to cases 7 to 9.53 Case 10 will be discussed later. As mentioned earlier, the MEMS wafer can be fabricated either with wire-bonding pads or TSV and solder bumps or a solder-bumped flip-chip, as shown in Figs. 2-42 through 2-44. These are followed by releasing (etching) the MEMS wafer and singulation. For 3D MEMS packaging with lateral electrical feed-through (cases 1, 2, and 3), there is no TSV in both the ASIC and cap wafers (see Fig. 2-42). In these cases, cavities should be formed in the cap wafer by either KOH etching or use of a laser. Then one performs the bonding of the MEMS device (chip) to the ASIC wafer (C2W). This
Advanced MEMS Packaging MEMS wafer
MEMS with wire-bonding pad
MEMS with TSV
MEMS with flip-chip
MEMS devices released
TSV formations and wafer bumping
Wafer bumping
Singulation
MEMS devices released
MEMS devices released
ASIC wafer without TSV
Singulation
C2W wire bonding
Singulation
C2W solder bonding
C2W solder bonding
Cap wafer without TSV
ASIC wafer to cap wafer bonding Cavity formation on cap wafer without TSV
Singulation
FIGURE 2-42 Assembly process for 3D MEMS packaging with lateral electrical feedthrough. MEMS wafer
ASIC wafer
MEMS with wire-bonding pad
MEMS with TSV
MEMS devices released
TSV formations and wafer bumping
Wafer bumping
Singulation
MEMS devices released
MEMS devices released
Singulation
Singulation
C2W solder bonding
C2W solder bonding
TSV formation on ASIC wafer C2W wire bonding
Cap wafer without TSV
ASIC wafer to cap wafer bonding Wafer bumping
Cavity formation on cap wafer
Singulation
FIGURE 2-43 Assembly process for 3D MEMS packaging with vertical electrical feed-through the TSV in an ASIC chip.
73
74
Chapter Two MEMS wafer
MEMS with wire-bonding pad
MEMS with TSV
MEMS with flip-chip
MEMS devices released
TSV formations and wafer bumping
Wafer bumping
Singulation
MEMS devices released
MEMS devices released
ASIC wafer without TSV
Singulation
C2W wire bonding
C2W solder bonding
Singulation
C2W solder bonding
Cap wafer without TSV
ASIC wafer to cap wafer bonding Cavity formation on cap wafer without TSV
Singulation
FIGURE 2-44 Assembly process for 3D MEMS packaging with vertical electrical feed-through the TSV in the package cap.
will be followed by bonding of the cavity-cap wafer to the ASIC wafer (W2W). Finally, the bonded wafers are singulated into individual units, which are ready to be wire bonded on the substrate of a package or on a PCB, as shown in Fig. 2-45. For both cases, encapsulant is recommended. For 3D MEMS packaging with vertical electrical feed-through in the ASIC chip (cases 4, 5, and 6), the TSV must be fabricated on the ASIC wafer before C2W bonding, as shown in Fig. 2-43. After the W2W (cap-to-ASIC) bonding, wafer bumping should be performed on the bottom side of the ASIC wafer. After singulations, the individual units can be soldered on the substrate of either a package or a PCB, as shown in Fig. 2-46. For the PCB case, underfill is necessary for the reliability of the solder joints. For the solder-bumped flip-chipin-package case, use of underfill depends on the substrate material. If it is made of ceramic, then underfill is optional. However, if it is an organic substrate, then underfill is a must. For 3D MEMS packaging with vertical electrical feed-through in the package cap (cases 7, 8, and 9), the TSV and cavity must be fabricated on the cap wafer before W2W bonding, as shown in Fig. 2-44. After W2W bonding, wafer bumping should be performed on the bottom side of the cap wafer. The rest is the same as in cases 4 through 6, and Fig. 2-47 shows an example of the complete 3D MEMS packaging with vertical electrical feed-through in the package cap.
Advanced MEMS Packaging Cavity-cap Sealing ring
Wire bonding MEMS device
ASIC chip Signal lines go through beneath sealing ring to wire-bonding pad on the chip periphery
Circuitry MEMS chip (substrate)
MEMS/ASIC module wire-bonding on the substrate of a package which is assembled on PCB
Bonding pad on a substrate or PCB
MEMS/ASIC module wire-bonding directly on PCB
Substrate
PCB
FIGURE 2-45 Complete 3D MEMS packaging with lateral electrical feed-through (encapsulants are recommended).
MEMS substrate with TSV Cavity-cap Sealing ring
MEMS device
ASIC chip
Ordinary solder bumps Tiny solder bumps
Through-silicon via (TSV)
MEMS/ASIC module attached on the substrate of a package which is assembled on PCB
MEMS/ASIC module flipchip attached on PCB
Substrate Solder balls PCB
FIGURE 2-46 Complete 3D MEMS packaging with vertical electrical feed-through in the TSV of a ASIC chip (underfills are recommended).
75
76
Chapter Two Ordinary solder bumps Cavity-cap
Sealing ring
Through-silicon via (TSV)
ASIC chip MEMS device
Solder bumps
MEMS substrate with solder bumps
MEMS/ASIC module attached on the substrate of a package which is assembled on PCB
MEMS/ASIC module flipchip attached on PCB
Substrate Solder balls PCB
FIGURE 2-47 Complete 3D MEMS packaging with vertical electrical feed-through the TSV of the package cap (underfills are recommended).
In the food chain of electronic products, packaging is a downstream process (i.e., the packaging people cannot be or are not in a proactive position and cannot say too much), and the packaging people just package whatever is given them by the semiconductor people (i.e., our job starts from the wafers). Case 10 (see Fig. 2-41) is a very low-cost, high-performance 3D MEMS package.53 However, in order to make it, the MEMS device (chip) must be much larger (to make space for the sealing ring) than that packages in cases 1 through 9 with a cavity cap. Thus, from a semiconductor points of view, this is a very bad idea because many fewer MEMS devices can be produced on the same size MEMS wafer.
References 1. Andry, P. S., Tsang, C. K., Webb, B. C., Sprogis, E. J., Wright, S. L., Bang, B., and Manzer, D. G. “Fabrication and characterization of robust through-silicon vias for silicon-carrier applications.” IBM Journal of Research and Development 52:571–581, 2008. 2. Knickerbocker, J. U., Andry, P.S., Dang, B., Horton, R. R., Patel, C. S., Polastre, R. J., Sakuma, K., Sprogis, E. S., Tsang, C. K., Webb, B. C., and Wright, S. L. “3-D silicon integration.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 538–543. 3. Kumagai, K., Yoneda, Y., Izumino, H., Shimojo, H., Sunohara, M., and Kurihara, T. “A silicon interposer BGA package with Cu-filled TSV and multilayer Cu-plating
Advanced MEMS Packaging
4.
5.
6. 7.
8. 9.
10.
11.
12.
13.
14. 15.
16.
17.
interconnection.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 571–576. Sunohara, M., Tokunaga, T., Kurihara, T., and Higashi, M., “Silicon interposer with TSVs (through-silicon vias) and fine multilayer wiring.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 847–852. Lee, H. S., Choi, Y.-S., Song, E., Choi, K., Cho, T., and Kang, S. “Power delivery network design for 3D SIP integrated over silicon interposer platform.” In IEEE Proceedings of Electronic Components and Technology Conference, Reno, NV, May 2007, pp. 1193–1198. Matsuo, M., Hayasaka, N., and Okumura, K. “Silicon interposer technology for high-density package.” In IEEE Proceedings of Electronic Components and Technology Conference, Las Vegas, NV, May 2000, pp. 1455–1459. Selvanayagam, C., Lau, J. H., Zhang, X., Seah, S., Vaidyanathan, K., and Chai, T. “Nonlinear thermal stress/strain analysis of copper filled TSV (through silicon via) and their flip-chip microbumps.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 1073–1081. Wong, E., Minz, J., and Lim, S. K. “Effective thermal via and decoupling capacitor insertion for 3D system-on-package.” In IEEE Proceedings of Electronic Components and Technology Conference, San Siego, CA, May 2006, pp. 1795–1801. Khan, N., Rao, V., Lim, S., Ho, S., Lee, V., Zhang, X., Yang, R., Liao, E., Ranganathan, N., Chai, T., Kripesh, V., and Lau, J. H. “Development of 3D silicon module with TSV for system in packaging.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 550–555. Ho, S., Yoon, S., Zhou, Q., Pasad, K., Kripesh, V., and Lau, J. H. “High rf performance TSV for silicon carrier for high frequency application.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 1956–1952. Premachandran, C., Rangnathan, N., Mohanraj, S., Chong Ser Choong, and Iyer, M. K. “A vertical wafer level packaging using through hole filled via interconnect by lift off polymer method for MEMS and 3D stacking applications.” In Proceedings of the Fifty-first Electronic Components and Technology Conference, Lake Buena Vista, FL, 2005, pp. 1094–1098. Chen, K. S., Ayon, A. A., Zhang, X., and Spearing, S. M. “Effect of process parameters on the surface morphology and mechanical performance of silicon surfaces after deep reactive ion etching (DRIE).” J. Microelectromech. Syst. 11:264–275, 2002. Zhang, X., Chai, T., Lau, J. H., Selvanayagam, C., Biswas, K., Liu, S., Pinjala, D., Tang, G., Ong, Y., Vempati, S., Wai, E., Li, H., Liao, B., Ranganathan, N., Kripesh, V., Sun, J., Doricko, J., and Vath, C. “Development of through silicon via (TSV) interposer technology for large die (21 × 21 mm) fine-pitch Cu/low-k FCBGA package.” IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 2009, pp. 305–312. Hu, G., Kalyanam, H., Krishnamoorthy, S., and Polka, L. “Package technology to address the memory bandwidth challenge for tera-scale computing.” INTEL Technol. J. 11:197–206, 2007. Knickerbocker, J. U., Andry, P. S., Buchwalter, L. P., Deutsch, A., Horton, R. R., Jenkins, K. A., Kwark,Y. H., McVicker, G., Patel, C. S., Polastre, R. J., Schuster, C., Sharma, A., Sri-Jayantha, S. M., Surovic, C. W., Tsang, C. K., Webb, B. C., Wright, S. L., McKnight, S. R., Sprogis, E. J., and Dang, B. “Development of next-gereration system-on-package (SOP) technology based on silicon carriers with fine-pitch interconnection.” IBM J. Res. Dev. 49:725–754, 2005. Tomita, Y., Morifuji, T., Ando, T., Tago, M., Kajiwara, R., Nemoto, Y., Fujii, T., Kitayama, Y., and Takahashi, K. “Advanced packaging technologies on 3D stacked LSI utilizing the micro interconnections and the layered microthin encapsulation.” In Proceedings of the Fifty-first Electronic Components and Technology Conference, Orlando, FL, 2001, pp. 353–360. Choi, W. K., Premachandran, C., Ong, C., Ling, X., Liao, E., Khairyanto, A., Chne, K., Thaw, P., and Lau, J. H. “Development of novel intermetallic joints
77
78
Chapter Two using thin film indium based solder by low temperature bonding technology for 3D IC stacking.” IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 2009, pp. 333–338. 18. Takahashi, K., Umemoto, M., Tanaka, N., Tanida, K., Nemoto, Y., Tomita, Y., Tage, M., and Bonkohara, M. “Ultra-high-density interconnection technology of three-dimensional packaging.” Microelectronics Reliability 43:1267–1279, 2003. 19. Lau, J. H., Lim, Y., Lim, T., Tang, G., Khong, C., Zhang, X., Ramana, P., Zhang, J., Tani, C., Chandrappan, J., Chai, J., Li, J., Tangdiongga, G., and Kwong, D. “Design and analysis of 3D stacked optoelectronics on optical printed circuit boards.” In Proceedings of SPIE, Photonics Packaging, Integration, and Interconnects VIII, San Jose, CA, January 19–24, 2008, Vol. 6899, pp. 07.1–07.20. 20. Lau, J. H., and Tang, G. “Thermal management of 3D IC integration with TSV (through silicon via).” IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 2009, pp. 635–640. 21. Yu, A., Kumar, A., Ho, S., Wai, H., Lau, J. H., Khong, C., Lim, S., Zhang, X., Yu , D., Su, N., Chew, M., Ching, J., Tan, T., Kripesh, V., Lee, C., Huang, J., Chiang, J., Chen, S., Chiu, C., Chan, C., Chang, C., Huang, C., and Hsiao, C., “Development of fine pitch solder microbumps for 3D chip stacking.” IEEE Proceedings of Electronic Packaging and Technology Conference, Singapore, December 2008, pp. 387–392. 22. Yu, A., Lau, J. H., Ho, S., Kumar, A., Wai, Y., Yu, D., Jong, M., Kripesh, V., Pinjala, D., Kwong, D., “Study of 15-μm-pitch solder microbumps for 3D IC integration.” IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 2009, pp. 6 –10. 23. Yu, A., Lau, J. H., Ho, S., Kumar, A., Yin, H., Ching, J., Kripesh, V., Pinjala, D., Chen, S., Chan, C., Chao, C., Chiu, C., Huang, M., and Chen, C., “Three dimensional interconnects with high aspect ratio TSVs and fine pitch solder microbumps.” IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 2009, pp. 350–354. 24. Yu, A., Khan, N., Archit, G., Pinjala1, D., Toh, K., Kripesh1, V., Yoon, S., and Lau, J. H. “Development of silicon carriers with embedded thermal solutions for high power 3D package.” IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 24–28. 25. Rebeiz, G. M. RF MEMS: Theory, Design and Technology. New York: Wiley, 2003. 26. Nguyen, C. “MEMS technology for timing and frequency control.” IEEE Trans. Ultrason. Ferroelect. Freq. Contr. 54:251–270, 2007. 27. Mohamed Gad-el-Hak. The Mems Handbook. Boca Raton, FL: CRC Press, 2002. 28. Hacker, J. B., Mihailovich, R. E., Kim, M., and DeNatale, J. F. “A Ka-band 3-bit rf MEMS true-time-delay network.” IEEE Trans. Microw. Theory Tech. 51:305–308, 2003. 29. Anagnostou, D. E., Zheng, G., Chryssomallis, M., Lyke, J., Ponchak, G., Papapolymerou, J., and Christodoulou, C. G. “Design, fabrication and measurements of a self-similar re-configurable antenna with rf-MEMS switches.” IEEE Transactions on Antennas Propagat. 54:422–432, 2006. 30. Liu, A. Q., and Zhang, X. M. “A review of MEMS external-cavity tunable lasers.” J. Micromech. Microeng. 17:R1–R13, 2007. 31. Huff, G. H., and Bernhard, J. T. “Integration of packaged rf MEMS switches with radiation pattern reconfigurable square spiral microstrip antennas.” IEEE Trans. Antennas Propagat. 54:464–469, 2006. 32. Van Caekenberghe, K., and Sarabandi, K. “A 2-bit Ka-band rf MEMS frequency tunable slot antenna.” IEEE Antennas and Wireless Propagat. Lett. 7:179–182, 2008. 33. Nguyen, C. “MEMS technology for timing and frequency control,” IEEE Trans. Ultrason. Ferroelect. Freq. Contr. 54:251–270, 2007. 34. Tan, G. L., Mihailovich, R. E., Hacker, J. B., DeNatale, J. F., and Rebeiz, G. M. “Low-loss 2- and 4-bit TTD MEMS phase shifters based on SP4T switches.” IEEE Trans. Microwave Theory Tech. 51:297–304, 2003. 35. Hacker, J. B., Mihailovich, R. E., Kim, M., and DeNatale, J. F. “A Ka-band 3-bit rf MEMS true-time-delay network.” IEEE Trans. Microwave Theory Tech. 51:305–308, 2003.
Advanced MEMS Packaging 36. Ford, J. E., Goossen, K. W. , Walker, J. A., Neilson, D. T., Tennant, D. M., Park, S. Y., and Sulhoff, J. W. “Interference-based micromechanical spectral equalizers.” IEEE J. Select. Topics Quantum Elect. 10:579–587, 2004. 37. Nordquist, C. D., Dyck, C. W., Kraus, G. M., Reines, I. C., Goldsmith, C. L., Cowan, W. D., Plut, T. A., Austin, F., Finnegan, P. S., Ballance, M. H., and Sullivan, C. T. “A dc to 10 GHz 6-BIT RF MEMS time delay circuit.” IEEE Microwave Wireless Component Lett. 16:305–307, 2006. 38. Perruisseau-Carrier, J., Fritschi, R., Crespo-Valero, P., and Skrivervik, A. K. “Modeling of periodic distributed MEMS application to the design of variable true-time-delay lines.” In IEEE Trans. Microwave Theory Tech. 54:383–392, 2006. 39. Lakshminarayanan, B., and Weller, T. M., “Design and modeling of 4-bit slowwave MEMS phase shifters.” IEEE Trans. Microwave Theory Tech. 54:120–127, 2006. 40. Lakshminarayanan, B., and Weller, T. M. “Optimization and implementation of impedance-matched true-time-delay phase shifters on quartz substrate.” IEEE Trans. Microwave Theory Tech. 55:335–342, 2007. 41. Van Caekenberghe, K., and Vaha-Heikkila, T. “An analog rf MEMS slotline true-time-delay phase shifter.” IEEE Trans. Microwave Theory Tech. 56: 2008. 42. Maciel, J. J., Slocum, J. F., Smith, J. K., and Turtle, J. “MEMS electronically steerable antennas for fire control radars.” IEEE Aerosp. Electron. Syst. Mgnt., November 2007, pp. 17–20. 43. Pranonsatit, S., Holmes, A. S., Robertson, I. D., and Lucyszyn, S. “Single-pole eight-throw rf MEMS rotary switch.” IEEE/ASME J. Microelectromech. Syst. 15:1735–1744, 2006. 44. Lin, L. Y., and Goldstein, E. L. “Opportunities and challenges for MEMS in lightwave communications.” IEEE J. Select. Topics Quantum Electron. 8:163–172, 2002. 45. Vaha-Heikkila, T., Van Caekenberghe, K., Varis, J., Tuovinen, J., and Rebeiz, G. M. “Rf MEMS impedance tuners for 6–24 GHz applications.” Wiley Int. J. RF Microwave Computer-Aided Engineering 17:265–278, 2007. 46. Schoebel, J., Buck, T., Reimann, M., Ulm, M., Schneider, M., Jourdain, A., Carchon, G. J., and Tilmans, H. A. C. “Design considerations and technology assessment of phased array antenna systems with rf MEMS for automotive radar applications.” IEEE Trans. Microwave Theory Tech. 53:1968–1975, 2005. 47. Wu, M. C., Solgaard, O., and Ford, J. E. “Optical MEMS for lightwave communication.” J. Ligtwave Technol. 24:4433–4454, 2006. 48. Mailloux, R. J. Phased Array Antenna Handbook. London: Artech House, 2005. 49. Hoffmann, M., and Voges, E. “Bulk silicon micromachining for MEMS in optical communication systems.” J. Micromech. Microeng. 12:349–360, 2002. 50. Jung, C., Lee, M., Li, G. P., and Flaviis, F. D. “Reconfigurable scan-beam singlearm spiral antenna integrated with rf MEMS switches.” IEEE Trans. Antennas Propagat. 54:455–463, 2006. 51. Premachandran, C. S., Chew, M., Choi, W., Khairyanto, A., Chen, K., Singh, J., Wang, S., Xu, Y., Chen, N., Sheppard, C., Olivo, M., and Lau, J. H. “Influence of optical probe packaging on a 3D MEMS scanning micro mirror for optical coherence tomography (OCT) applications.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 829–833. 52. Premachandran, C. S., Lau, J. H., Ling, X., Khairyanto, A., Chen, K., and Myo Ei Pa Pa. “A novel, wafer-level stacking method for low-chip yield and non-uniform, chip-size wafers for MEMS and 3D SiP applications. In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 314–318. 53. Lau, J. H. “3D MEMS packaging.” In IMAPS Proceedings, San Jose, CA, November 2009. 54. Chen, K., Premachandran, C., Choi, K., Ong, C., Ling, X., Ratmin, A., Pa, M., and Lau, J. H. “C2W low temperature bonding method for MEMS applictions.” In IEEE Proceedings of Electronics Packaging Technology Conference, Singapore, December 2008, pp. 1–7.
79
This page intentionally left blank
CHAPTER
3
Enabling Technologies for Advanced MEMS Packaging 3.1 Introduction As discussed in previous chapters, through-silicon vias (TSVs); wafer thinning; thin-wafer strength measurements; thin-wafer handling; chip-to-chip (C2C), chip-to-wafer (C2W), and wafer-to-wafer (W2W) bonding; and microelectromechanical systems (MEMS) wafer dicing are key enabling technologies for advanced MEMS packaging. This chapter presents TSVs, piezoresistive stress sensors, wafer thinning and thin-wafer handling, low temperature bonding, and MEMS wafer dicing. In order to make and ship green MEMS products everywhere in the world, these products must be compliant with the Restriction of the Use of Certain Hazardous Substances (RoHS) directive (e.g., lead free). Thus RoHS requirements, such as the fact that MEMS packaging must be lead-free and their lead-free solder joints must be reliable, will be discussed briefly.
3.2 TSVs for MEMS Packaging For three-dimensional (3D) MEMS packaging, TSVs are the most important enabling technology. TSVs provide advanced vertical interconnects and system-in-package (SiP) solutions such as C2C, C2W, and W2W stacking; wafer-level packaging and redistribution; interposer packaging; and the shortest electrical path (vertical electrical feedthrough) between two sides of a silicon “chip.” Just as with many other new technologies, TSVs still face many critical issues. In the development of TSVs, the following must be noted and understood.1–21
81
82
Chapter Three • TSV cost is higher than that of wire bonding. • The only TSV volume product is CMOS image sensors. • Memory (e.g., Flash, DRAM, and SRAM) have just been talked about. • High-speed logic (e.g., processors and FPGAs) will come even later. • High-volume production tools are lacking and/or expensive. • TSV design guidelines are not commonly available. • TSV design software is lacking. • TSV technology usually requires redistribution layers (RDL). • TSV technology usually requires microbumps. • Test methods and software for TSVs are lacking. • Copper filling helps on thermal problems but increases thermal coefficient of expansion (TCE). • Copper filling takes a long time (low throughputs). • TSV wafer yields are high (>99.8 percent) owing to the large number of vias. • TSV wafer warpage is a problem owing to TCE mismatch. • Thin-wafer handling is necessary during all processes. • TSVs with high aspect ratios are difficult to make. • TSV inspection methodology is lacking. • TSV expertise is lacking. • TSV infrastructure is lacking. • TSV standards are lacking. Over the past few years, some of these critical issues have been studied by a number of experts. Their results have already been disclosed in various journals or, more incidentally, in the proceedings of a number of conferences, symposia, and workshops whose primary emphases are electrical packaging and interconnection.1–21 Consequently, there is no single source of information devoted to the state of the art of TSV technology. This chapter discusses only the five key TSV process steps, and they are demonstrated through the vias-first process.
3.2.1 Via Formation The vias in a silicon wafer can be formed either by etching (wet process) or by laser drilling (dry process). Reviewing the literatures, more than 80 percent of vias have been formed by deep reactive-ion etching (DRIE), which is a highly anisotropic etching process. However,
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g 10000 Laser-A Laser-B Laser-C Laser-D DRIE-A DRIE-B DRIE-C DRIE-D
Cost ($/w)
1000
100
10 10
100
1000
10000
# Vias/die
FIGURE 3-1 Sematech’s cost model for fabricating TSVs by laser and by DRIE.
based on Sematech’s cost model of DRIE versus laser (Fig. 3-1), it can be seen that for lower numbers of vias per die, laser drilling may be cheaper. In addition, vias made by laser are adequate for most of applications of MEMS packaging. For example, Fig. 3-2 shows the vias of a cap wafer made by laser.20 Furthermore, the cavity of a cap
TSV
Cross section of cap wafer by laser machining
Cross section of cap wafer by laser machining
Cross section of cap wafer by KOH (potassium hydroxide) wet etch
FIGURE 3-2 MEMS cap wafer with cavity and TSV fabricated by laser and by KOH etch methods.
83
84
Chapter Three wafer can be made by laser machining, even though KOH etch yields a better (straight) wall condition. In this chapter, however, the threestep method developed14,16,18 based on the high-rate DRIE BOSCH technology will be discussed. The silicon vias are formed in an inductive-coupled plasma (ICP)–based deep reactive ion etching system from Surface Technology Systems (STS). Although the STS ICP system is designed mainly for performing deep reactive-ion etching of silicon by a specially designed switched etch and passivation process, also known as the BOSCH process, it also can be used in reactive-ion etch mode, referred as the non-BOSCH process.18 The system consists of ICP electronics, loadlock and carousel wafer-loading unit, and a process chamber. The plasma is generated by a coil assembly that is inductively coupled at 13.56 MHz via the matching unit in a ceramic plasma chamber. This provides high-density plasma capable of achieving high etch rates with little substrate damage. Independent biasing of the platen is made available by a separate 13.56-MHz radiofrequency (RF) biasing circuit on the bottom electrode that comes with automatic power control and impedance matching. Process gas is introduced to the chamber through the upper electrode assembly. Wafers are clamped by electrostatic chuck (ESC) on the lower electrode, which is powered at 13.56 MHz. The platen temperature is kept at 10°C by using recirculating deionizer (DI) water through a chiller system. The high-aspect-ratio tapered silicon vias are formed by three independently controlled process steps: (1) the straight via formation step by the BOSCH etch process, (2) the via tapering step by a controlled isotropic etch process, and (3) the corner-rounding step by a global isotropic etch process. The first etching step is designed mainly to achieve high etch rates with the BOSCH etch process. Typically, a high-etch-rate BOSCH process tends to give a vertical to slightly reentrant profile, as shown in Fig. 3-3 (left). The gases used in the BOSCH process are mainly sulfur hexafluoride (SF6) plus oxygen (O2) in the etch phase and C4F8 in the passivation phase. The recipes are shown in Table 3-1.18 It should be noted that as a consequence of the cyclic etch/passivation process, the sidewalls become scalloped or rough. In this step, the via is etched to approximately 50 to 60 percent of the final depth. This step defines the dimension of the via at the bottom and the depth. A non-BOSCH etch process consisting of a reactive-ion etching (RIE) process is used to produce the required tapered-sidewall profile. This is basically a controlled isotropic etch process that uses SF6 plus O2 plus Ar (argon) etch chemistry (see Table 3-1). The oxygen used helps in sidewall passivation and also controls excessive lateral etch rate. A proper balance between SF6 and O2 provides the desired taper angle to the via structure. As a consequence of this process, a sharp curvature is formed at the top of the via, as shown in Fig. 3-3 (center). At the end of step 1 (BOSCH process) and step 2 (non-BOSCH process),
108.1 µm
62.2 µm
137.82 µm 91.48 µm
96.5 17.05 µm
210µm
57.3 µm
After step 1 (BOSCH)
222µm
55.3 µm
220.45 µm
After step 2 (RIE)
55.11 µm
After step 3 (isotropic)
FIGURE 3-3 Step 1 shows the results achieved after 50-μm-diameter vias are etched to a depth in the range of 200 to 220 μm. Step 2 shows the evolution of a tapered profile after etch by a controlled-isotropic etch process and step 3 shows the final tapered via profile after the top corner is rounder by a global isotropic etch process.
Step 1: Straight (BOSCH) etch process
Etch cycle: APC: 77% (26 mt); 130 sccm SF6; 13 sccm O2; 600-W coil power; 20-W platen power; 6 seconds Passivation cycle: APC: 77% (17 mt); 85 sccm C4F8; 600-W coil; 5 seconds Platen temperature: 10°C Total process time: 60 minutes Etch rate: 3 to 3.5 μm/min on 15% to 20% exposed area
Step 2: Via tapering (RIE) process
APC: 78% (30 mt); 84 sccm SF6; 67 sccm O2; 59 sccm Ar; 600-W coil power; 30-W platen power Platen temperature: 10°C Process time: 60 minutes Etch rate: 3.5 to 4.0 μm/min on 15% to 20% exposed area
Step 3: Via corner rounding (isotropic etch) process
APC: 65% (12 to 13 mtorr); 180 sccm SF6; 18 sccm O2; 600-W coil power; 30-W platen power Platen temperature: 10°C Process time: 10 minutes Etch rate: 1.5 to 2.0 μm/min on blanket silicon wafer
TABLE 3-1
Summary of the Three-Step Via Tapering Process
85
86
Chapter Three the required via depth and taper angle are almost achieved, except for the sharp curvature at the top of the via. After completing the earlier two etch steps, the etch mask is fully stripped and cleaned. The wafer then is subjected to a maskless global isotropic etch process. In this etch step, the etched via patterns are mainly subjected to an isotropic etch plasma that is rich in fluorine radical (see Table 3-1 for the recipes). Since the reaction in this step is mainly chemical in nature and mostly diffusion-limited, the reaction occurs more on the rough edges and sharp corners in the top region of the microstructure, resulting in well-rounded, smooth sidewalls inside the vias, as shown in Fig. 3-3 (right).
3.2.2
Dielectric Isolation Layer (SiO2) Deposition
The thermal oxidation (wet process) is used to deposit the isolation layer. The 1-μm SiO2 is grown in a Micro Fabrication Laboratory (MFL) furnace. Hydrogen and oxygen are mixed in the quartz bulb, where they react to create a flame and steam at 1050°C. The oxidation time of Si is 3-½ hours. Conformal SiO2 is shown in Fig. 3-4. The top, middle, and bottom of the via are covered by uniform SiO2. Uniformity of SiO2 is within ±5 percent. The sidewall roughness decreases from 200 to 250 nm to less than 100 nm because of silicon consumption in wet oxidation.18 The SiO2 also can be deposited by the dry process—plasma-enhanced chemical vapor deposition (PECVD), as shown in Fig. 3-5. It can be seen that the deposited oxide thickness is 1.9 to 2 μm on the top side of the via, 1.3 to 1.4 μm on the top sidewall, 0.7 to 0.8 μm on the middle sidewall, and 0.35 to 0.45 μm on the via bottom. Thus, the SiO2 thickness made by the dry process is not as uniform as that made by the wet process. In this case, the process temperature is less than 250°C.18 Top Top Middle
Middle
Bottom of via Bottom Bottom
FIGURE 3-4 Dielectric isolation layer (SiO2) deposited by wet thermal oxidation (1080°C).
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Top
Middle
Bottom
FIGURE 3-5 Dielectric isolation layer (SiO2) created by plasma deposition
(<250°C).
3.2.3
Barrier/Adhesion and Seed Metal Layer Deposition
Figure 3-6 shows the Ti (3000-Å) barrier and Cu (2-μm) seed layer on the walls of the via. They are deposited by physical vapor deposition (PVD) with Tango System’s AXCECA chamber, and the key process parameters are shown in Table 3-2. It can be seen that very good coverage at via bottom and via sidewall has been achieved.14
143 nm
Bottom 2.jpg
Lower wall region showed thicker coverage than middle wall due to a higher flux of resputtered material being collected. The bottom shows finer grain structure, most likely from ion bombardment.
FIGURE 3-6 Ti barrier/adhesion layer and Cu seed layer created by Tango AXCECA physical vapor deposition.
87
88
Chapter Three Process
Ti
Cu
Thickness
3 kÅ
2 µm
Dc power
8 kW
8 kW
Coil power
600 W
600 W
Bias power
1000 W
1000 W
Ar flow/ch. pressure
10/1.5 mT
20/2 mT
Bias voltage
100 V
150 V
Target voltage
550 V
630 V
TABLE 3-2 Important Process Parameters for Fabricating the Ti Barrier and Cu Seed Layer
The Ti barrier and Cu seed layer also can be deposited by a wet process. Depositions of the insulation and barrier layers inside highaspect-ratio TSVs have been achieved by Alchimer’s electrografting (eG), which initiates chemical bond formation by means of a small electric current, followed by electroless chemical propagation. Figure 3-7 shows the results of wet deposition, and it can be seen that good coverage on via sidewalls and via bottom has been achieved. (Ti = 100 nm and Cu = 1 μm).
FIGURE 3-7 Ti barrier/adhesion layer and Cu seed layer deposited by Alchimer’s electrografting.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
3.2.4 Via Filling The via can be filled with Cu, Ti, Al, or solder by electroplating, W by sputtering, or polymers by printing with the help of vacuum. Based on the literatures, most of the vais are filled by electroplating the Cu, which will be discussed in this book. The Cu electroplating solution for deep and high-aspect-ratio viafilling application can be either copper sulfate or cyanide-based.14,16,18 Typical composition of an electrolyte includes CuSO4, H2SO4, Cl−, with additives including suppressor, accelerator, and leveler. The electroplating system used for deep via filling is a research system from Rena. Finally, void-free wafer-level Cu filling for 300-μm-deep vias has been achieved, as shown in Figs. 3-8 through 3-10. It should
FIGURE 3-8 Cu overburden owing to long plating time.
FIGURE 3-9 Chemical and mechanical polishing (CMP).
89
90
Chapter Three
(a) Cross-section of TSV with seams
3D x-ray image with the CT (computed tomography) reconstruction of the electroplated Cu (b)
Seams/voids
FIGURE 3-10 (a) 2D x-ray image of the electroplated Cu (wafer tilted at 70 degrees). (b) 3D x-ray image with the computed tomographic (CT) reconstruction of the electroplated Cu with seams/voids. (c) 3D x-ray image with the CT reconstruction of the Cu-filled void-free TSV (Ref. 14).
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
SEM image showing void-free electroplated Cu vias 3D x-ray with CT (computed tomography) reconstruction for Cu-filled TSVs (c)
FIGURE 3-10 (Continued)
be noted that plating chemistry, low plating current, and pretreatment (i.e., wetting + DI rinsing + preabsorbing accelerator) are the key contributors to void-free Cu filling for deep and high-aspect-ratio tapered vias. The electroplating process uses pulsed reverse plating, which employs a two-component additive system consisting of brightener and leveler. TSV quality is inspected by the 2D and 3D x-ray nondestructive testing (NDT) at an earlier stage in the fabrication process. In other words, both 2D and 3D x-ray tests are used to monitor and check TSV quality during the fabrication process without resorting to physical cross-sectioning. Figure 3-10a shows a 2D x-ray image at a tilted angle of 70 degrees for through-view of the Cu-filled TSV array in the wafer. Figure 3-10b shows a 3D x-ray with computed tomographics (CT) reconstruction of the Cu-filled TSVs with seams/voids. After process improvements, Figure 3-10c shows a 3D x-ray with CT reconstruction of the Cu-filled void-free TSVs.14
3.2.5
Cu Polishing by Chemical/Mechanical Polish (CMP)
A thick layer (30 to 50 μm) of Cu overburden (see Fig. 3-8) is plated on the wafer surface because of the long plating time required to fill the 300-μm-deep vias. The wafer bows because of the thick Cu on the surface. Conventional chemical etching takes a long time to remove the thick Cu, and nonuniform etching has been observed. Okamoto GNX 200 is used for the higher-stress Cu CMP. A soft polishing pad and strong-removal-rate slurry from Rohms and Hass are applied for thicker copper removal. The load of polishing is 320 to 350 g/cm2. The speed of pad and chuck are 90 rev/min (rpm). The speed of slurry
91
92
Chapter Three feeding is 170 to 200 ml/min. Figure 3-9 shows a cross section of a polished wafer with Cu-filled vias.
3.2.6
Fabrication of an ASIC Wafer with TSVs
As mentioned in Chapter 2, for 3D MEMS packaging with vertical electrical feed-through, one option is to have the ASIC wafer fabricated with TSVs.14,16,18 Figure 3-11 illustrates the TSV ASIC wafer fabrication and integration flow. After the deep vias are etched, insulated, filled with Cu metal, and polished by CMP during the earliest stage of fabrication (see Secs. 3.2.1 through 3.2.5), the front-side metallization and Cu-Ni-Au under-bump metallurgy (UBM) are built on top of the wafer. Next, the wafer is attached to a supporting wafer using a temporary adhesive material from Brewer Science, followed back-grinding (thinning) and backside processing to expose the vias. The bonded wafers then are processed for back-end metallization/UBM/solder bumps. The backside UBM is electroplated copper. The solder-bump material is SnAgCu (SAC). After all these processes, the bonded wafers are debonded by sliding the wafers apart at higher temperature (200°C). Temporary bonding and debonding of wafers can be done with the EV Group equipment, which will be discussed in Sec. 3.4.2.
1. Via etch 6. Support wafer bonding
2. Oxide/barrier/seedlayer deposition
7. Via exposing by thinning
3. Cu via plating
8. Backside metallization/UBM
4. Cu CMP
TSV wafer 9. Solder bumping
5. Front-side metallization/UBM
Debonding
10. Debonding & cleaning
FIGURE 3-11 TSV wafer fabrication process and integration flow.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Now the TSV ASIC wafer, as shown in Fig. 3-11, is ready for the MEMS device (C2W) bonding or the MEMS wafer (W2W) bonding, which will be discussed in Sec. 3.5. After capping and dicing (which will be discussed in Sec. 3.6), the whole 3D MEMS SiP is ready to be mounted on the substrate of a package or a printed circuit board (PCB).
3.2.7
Fabrication of Cap Wafer with TSVs and Cavity
For vertical electrical feed-through MEMS packaging, the TSVs on the cap wafer could be fabricated more cheaply by laser drilling, as mentioned in Sec. 3.2.1, and this is shown in Fig. 3-2.20 The advantage of laser drilling is that it is a maskless and dry process, but the disadvantage is that it creates a rough surface that may affect TSV electrical performance. After via formation, the TSV is filled with conductive materials such as copper and conductive polymers. The cavity on the cap wafer also can be fabricated by laser drilling. However, most of the cavities fabricated today are done by the potassium hydroxide (KOH) wet etch process. It can be seen from Fig. 3-2 that this process provides a much smoother surface than laser drilling.20 The etch rate depends on the doping and crystallographic orientation of the silicon, as well as the concentration of KOH used. Usually the rate is 1 μm/min.
3.3
Piezoresistive Stress Sensors for MEMS Packaging Silicon piezoresistive stress sensors are powerful tools for in situ stress measurement.22–34 For advanced MEMS packaging, they can be used for measuring the strength of the MEMS wafer, the ASIC wafer, and the cavity-cap wafer during and after all the processes such as wafer thinning, SiO2 deposition, metallization, and electroplating. This section discusses the design, fabrication, calibration, and use of a piezoresistive stress sensor to measure the strength of wafers after mounting on a dicing tape and wafer thinning.
3.3.1 Design and Fabrication of Piezoresistive Stress Sensors The layout of a n-type stress-sensor design is shown in Figs. 3-12 and 3-13.32,34 The sensors R1, R2, R3, and R4 are fabricated along the [110], ⎡⎣100⎤⎦,⎡⎣110⎤⎦, and [010] directions of a p-type (100) silicon wafer. The resistance of the R1 and R3 sensors is about 0.625 kΩ, and that of the R2 and R4 resistors is about 0.932 kΩ. The sheet resistance of all the sensors is about 178 Ω/ . These n-type stress sensors are fabricated on the silicon wafer using the conventional process. First, a 4100-Å (100-Å thermal and then 4000-Å plasma-enhanced chemical vapor deposited) silicon dioxide is grown on the p-type silicon wafer. Then the oxide is etched from the area where the sensors are designed to be fabricated. After etching the
93
94
Chapter Three
y [100] '
y [110]
x '[010] x [110]
R1
R4
R3
R2
FIGURE 3-12 Piezoresistive stress-sensor rosette.
oxide, arsenic is implanted on the p-type silicon wafer to form the n-type resistor or sensor. The surface concentration of the dopant is around 1x10−3 cm. After forming the n-type resistor, 5000-Å plasma-enhanced chemical vapor deposition (PVCVD) oxide is deposited on the wafer, and then contact windows are opened in the oxide for resistors. Finally, TaN and Al metallizations are deposited to form metal contacts to the resistors, metallization lines, and probing pads. Figure 3-13 is a drawing of the sensor chip showing the metallization lines and probing pads. Four sensor rosettes are fabricated at different locations on a 5 × 5 mm chip.
FIGURE 3-13 Fabricated stress-sensor chip showing the metallization lines and probing pads.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
3.3.2
Calibration of Stress Sensors
The two basic requirements for piezoresistive stress sensors to perform stress measurements are (1) a measurable resistance change of sensors with the application of loads and (2) a sensor calibration to determine the piezoresistive coefficients.23 Sensor calibration involves measuring the resistance change of sensors with the application of a known stress and then determining the piezoresistive coefficients using the theory of piezoresistivity.23,25,26 Based on the theory of piezoresistivity, if an uniaxial stress σx is applied in the [110] direction of the sensor rosette shown in Fig. 3-12, then the piezoresistive coefficients are given by
∏ 11 + ∏ 12 =
∏ 44 =
1 ⎛ ΔR1 ΔR3 ⎞ + R30 ⎟⎠ σ x ⎜⎝ R10
1 ⎛ ΔR1 ΔR3 ⎞ − R30 ⎟⎠ σ x ⎜⎝ R10
(3-1)
(3-2)
where ΔRi and Ri0, respectively, are the stress-induced resistance change and the initial resistance of the ith sensor. Once the values of the piezoresistive coefficients are known (and assuming the case of plane stress, σz = 0), piezoresistive sensors can be used to determine the unknown in-plane stress components (σx and σy) by measuring the change in resistance of sensors ΔRi and Ri0.23,25,26 Thus
⎛ ΔR ⎛ ΔR R3 ⎞ Δ R3 ⎞ ΔR ∏ 44 ⎜ 1 + + (∏ 11 + ∏ 12 ⎜ 1 − R30 ⎟⎠ R30 ⎟⎠ ⎝ R10 ⎝ R10 σx = 2 ∏ 44 (∏ 11 + ∏ 12
) )
⎛ ΔR ⎛ ΔR R3 ⎞ Δ R3 ⎞ ΔR ∏ 44 ⎜ 1 + − (∏ 11 + ∏ 12 ⎜ 1 − ⎟ ⎟ R R R R ⎝ 10 ⎝ 10 30 ⎠ 30 ⎠ σy = 2 ∏ 44 (∏ 11 + ∏ 12
) )
(3-3)
(3-4)
Various methods, such as four-point bending (4PB) of a strip of sensor chips,24,26–30 4PB of a sensor chip,31 a wafer-level vacuum chuck,30 and a hydrostatic load,24 have been used to calibrate piezoresistive stress sensors. In this section, the 4PB method with a strip of sensor chips is used for the calibration owing to its simple setup and more literature data24,26–30 for reference. Figure 3-14 shows the strip of sensor chips for the calibration of the piezoresistive stress sensors. It can be seen that the size is 70 × 10 mm and that there are 28 sensor chips in two rows. However, only the sensor rosette that is located at the center of the strip is used for calibration.
95
96
Chapter Three Area of interest
2F Stresssensor strip
t d
L
FIGURE 3-14 Piezoresistive coefficients determined by the stress-sensor strip with 4PB and an Instron microtester.
In order to perform the 4PB of the strip of sensor chips, a 4PB fixture and a loading machine to apply the load on the strip, a microscope to visualize the probing pads, two microprobes to probe the sensor pads, and a multimeter to measure the sensor’s resistance, as shown in Fig. 3-14, are needed. Here, an Instron microtester with a 100-N load cell is used to apply a given force (2F) on the strip. The relationship between the stress (σ) and applied force (2F) is reported in ref. 26. Thus σ=
3 F (L − d) t2 h
(3-5)
This equation is derived from the classical strength of material (beam theory) assuming a uniform bending stress state for points within the supports of the specimen. In this equation, L is the loading span, d is the supporting span, h is the width of the strip, and t is the thickness of the strip (chip). This formula works well if the deflection of the strip owing to the load is small and the t and h are small compared with the d and L.29 Thus, in the present work, L, d, h, and t are chosen to be of 50, 20, 10, and 0.73 mm, respectively. In the calibration process, first the resistance of the stress sensors is measured without any applied load. Then a given load (with an increment of 4 N up to 24 N) is applied on the strip using the 4PB fixture and Instron microtester, and the corresponding resistances of the stress sensors are measured with the help of the microprobe and multimeter. Considering the variation in the readings, at least eight strips of sensors from two different wafers are taken to calculate the average values.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g 1.2 R1 R2 R3 R4
Resistance, kohm
1.0
0.8
0.6
0.4 0
50 100 150 Applied stress, MPa
200
FIGURE 3-15 Resistances of stress sensors as a function of applied stress.
Figure 3-15 shows the resistances of sensors as a function of the applied stress. It can be seen that the resistance of n-type sensor decreases with an increase in applied stress. To determine the piezoresistive coefficients from the resistance versus applied stress data, according to Eqs. (3-1) and (3-2), slops of plots between normalized resistance changes (i.e., ΔR 1/R 10 ± ΔR 3/R 30) and applied stress, as shown in Fig. 3-16, are measured and tabulated in Table 3-3. The piezoresistive coefficients ∏11 + ∏12 and ∏44 of the n-type sensor are found to be –1.98 × 10−4 and –1.06 × 10−4 MPa−1, respectively.
Normalized resistance change
0.01 (ΔR1/R10 + ΔR3 /R30)
0.00
(ΔR1/R10 – ΔR3 /R30)
–0.01 –0.02 –0.03 –0.04 –0.05 –0.06 0
50
100
150
200
Applied stress, MPa
FIGURE 3-16 Normalized resistance change of stress sensors as a function of applied stress.
97
Chapter Three ∏11 + ∏12
−1.98 × 10−4 MPa−1
∏44
−1.06 × 10−4 MPa−1
TABLE 3-3 Piezoresistive Coefficients of n-Type Stress Sensor
These values of piezoresistive coefficients are in agreement with previously reported work.23 Once the piezoresistive coefficients ∏11 + ∏12 and ∏44 of the n-type stress sensor are determined, the stresses (σx and σy) can be calculated from Eqs. (3-3) and (3-4) with the measured change in resistance (ΔRi) and initial resistance (Ri0). In this chapter, the piezoresistive stress sensors will be used to evaluate the stresses in wafers after mounting of a dicing tape and thinning (back-grinding).
3.3.3
Stresses in Wafers after Mounting on a Dicing Tape
Figure 3-17 shows a 400-μm-thick sensor wafer mounted on a dicing tape with a dicing ring. It can be seen that a commercially available dicing tape is mounted or laminated on the backside of the wafer using a dicing ring and an automatic tape laminator (Dyna Tech).
FIGURE 3-17 Stresses in thinned sensor wafer after mounting on the dicing tape.
80
σx σy
60 Stress, MPa
98
40 20 0
–20 –40 400
300 200 Wafer thickness, μm
100
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g The parameters of the lamination process include a pressure of 0.3 MPa, a speed of 10 mm/s, a tape thickness of 70 mm, and lamination at room temperature (RT). After tape mounting, the wafer is baked at 70°C for 15 minutes to increase the adhesion between the dicing tape and the wafer. After baking, the dicing ring and any excess dicing tape are removed from the tape-mounted sensor wafer. The resistance measurement is performed at nine locations on a wafer, as shown in Fig. 3-18. The in-plane stress components (σx and σy) are determined by Eqs. (3-3) and (3-4), and their average values are shown in Fig. 3-17. It can be seen that the dicing-tape mounting increases the tensile stress at the surface of the sensor wafer. Owing to this increase in tensile stress, the stress in the 400-μm-thick wafer is in tension, whereas the stress in the 100-μm-thick wafer is still in compression, but its magnitude decreases significantly. The presence of these tensile and compressive stresses in the dicing-tape-mounted wafer is further confirmed with the wafer bending profile and bow values (by using 33-point measurements), as shown in Fig. 3-19 and Table 3-4, respectively. The transition in stress state in the sensor wafer after mounting with dicing tape can be explained through the dicing-tape mounting process. The dicing-tape mounting process is actually a lamination process, in which a polymer tape is stretched and laminated on the backside of the wafer. After that, the dicing tape tries to return to its
3
4
5
2
1
9
8
6
7
FIGURE 3-18 Stress-measurement locations on a stress-sensor wafer.
99
100
Chapter Three W
E
S
N
NW
SE
SW
NE
W
E
S
N
NW
SE
SW
NE
FIGURE 3-19 Bow data and bending profiles of a 400-μm-wafer (top) and a 100-μmwafer (bottom) after dicing-tape mounting.
Wafer Thickness (mm)
Bow (mm)
400
21.5
200
−20.8
100
−29.5
TABLE 3-4
Wafer Bow of Stress-Sensor Wafers of Different Thicknesses after Mounting with Dicing Tape
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g original shape owing to its viscoelastic behavior. Thus, after the lamination process, the shrinkage in dicing tape results in the development of a downward bending force on the sensor wafer, and therefore, the top surface of the wafer experiences a tensile stress.
3.3.4
Stresses in Wafers after Thinning (Back-Grinding)
In order to study the effects of wafer thinning on the strength of the wafer, three original sensor wafers (730 μm) were thinned down to three different thicknesses, namely, 400, 200, and 100 μm. A commercial back-grinding machine (Okamoto GNX 200) was used for the thinning process, which consisted of three major tasks: rough grinding, fine grinding, and polishing. The process parameters for the meshsize grinding wheel, spindle speed, chuck table speed, and feed rate are, respectively, No. 600, 3000 rpm, 230 rpm, and 180 to 190 mm/min for rough grinding and No. 2000, 3400 rpm, 230 rpm, and 12 to 16 mm/min for fine grinding. The final polishing is with a 200-ml/min slurry flow, 150-g/cm2 load, 230-rpm pad speed, and 210-rpm chuck speed. After thinning of the wafers, a resistance measurement is done at the same nine locations (as shown in Fig. 3-18) on the sensor wafer, and the stress components (σx and σy) are determined by Eqs. (3-3) and (3-4) and are shown in Table 3-5 for the case of a wafer thinned down to 100 μm. It can be seen that a large amount of compressive stress has been generated in the sensor wafer after thinning. Figure 3-20 shows the average stress as a function of wafer thickness, and it is apparent that the amount of in-plane stress (compressive) increases exponentially with a decrease in wafer thickness.
Location No.
Stress σx (MPa)
Stress sy (MPa)
1
−16
−23.6
2
−47.3
−24.6
3
−112
−89.2
4
−71.6
−48.8
5
−51.9
−44.3
6
−47.3
−24.6
7
−51.9
−44.3
8
−79.7
−56.9
9
−27.6
−20.0
Average
−56.1
−41.8
TABLE 3-5
Stress Components Measured at Different Locations on a Wafer after Thinning Down to 100 µm
101
Chapter Three
σx
20
σy 0 Stress, MPa
102
–20 –40 –60 –80 700
600
500
400
300
200
100
Wafer thickness, μm
FIGURE 3-20 Stress versus wafer thickness.
The degree of compressive stress on the sensor wafer is further confirmed by measuring the wafer bending profile and the bow of the original and back-ground wafers. The wafer bow was measured using the 33 point measurements and the results are shown in Fig. 3-21. The measured values are listed in Table 3-6. Transition of the wafer bow from positive to negative indicates that the stress state at sensor wafer plane changed from tensile to compressive. This transition in stress state can be understood with the help of sensor wafer processing materials. Basically, the sensor wafer consists of two layers of materials. The first layer (bottom layer) is a single-crystal silicon, and the second layer (top layer) is mainly 9000 Å of PECVD silicon dioxide. This PECVD silicon oxide is deposited on the silicon wafer at approximately 400°C. Thus, when the sensor wafer cools down to the RT, because of the thermal-expansion mismatch between the thin silicon dioxide [thermal expansion coefficient (TEC) = 0.54 ppm/K34] layer and the silicon substrate (TEC = 3.07 ppm/K34), it creates a bending (bowing upward) of the composite sensor wafer that generates tensile stress on top of the wafer. This is confirmed with the bow-measurement results shown in Fig. 3-21 (top). However, in order to define the reference point for stress measurement, the stress state on original wafer surface at RT is assumed as “stress free.” Thus, if the tensile stresses on the sensor-wafer surface decrease, then the stress sensor will detect an increase in compressive stress. The increase in compressive stress (decrease in tensile stress) in the thinned wafer can be attributed to the decrease in bending stiffness (which is to the cube of the thickness) of the silicon layer with the decrease in its thickness.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g W
E
S
N
NW
SE
SW
NE
W
E
S
N
NW
SE
SW
NE
FIGURE 3-21 Bow data and bending profiles of original (730-μm) wafer (top) and 100-μm thinned wafer (bottom).
Wafer Thickness (mm)
Bow (mm)
730 (original)
8.1
400
9.9
200
−3.9
100
−9.2
TABLE 3-6 Bow of Stress-Sensor Wafer Showing a Transition from Positive Bow to Negative Bow with a Decrease in Wafer Thickness
103
104
Chapter Three Compounded with the thermomechanical stresses imposed during the wafer back-grinding process, subsurface damage could occur on the backside of the silicon layer.
3.4 Wafer Thinning and Thin-Wafer Handling In order to have low-profile products with 3D MEMS packaging, the thickness of the chips/wafers (e.g., MEMS device, ASIC chip, and cap) is usually very thin. Making the wafer thin is not a big problem. Most of the back-grinding machines (e.g., Disco) can do the job and grind the wafers to as thin as 5 μm. However, handling thin wafers through all the semiconductor fabrication and packaging assembly processes is difficult. Usually, the thin-device wafer is temporarily bonded on a support wafer. Then it goes through all the semiconductor fabrication processes, such as metallization, passivation, and UBM, and the packaging processes, such as backgrinding and solder bumping. After all these are done, removing the thin wafer from the support wafer poses another big challenge. This section discusses a few methods for handling thin wafers.
3.4.1
3M Wafer Support System
Figures 3-22 and 3-23 show the new 3M wafer support system,35 which enables conventional back-grinding equipment to be used to produce wafers with a final thickness as low as 20 μm. The key to the
FIGURE 3-22 3M wafer support system with a wafer.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
FIGURE 3-23 3M wafer support system with a glass supporting plate.
3M system is its ability to provide a rigid, uniform support surface to minimize stress on the wafer as the silicon is removed, resulting in less cracking and chipping. The system includes both the equipment and consumables [3M UV-Curable Liquid Adhesive LC-2201, glass support plate (typically recycled, can be reused many times), and 3M light-to-heat Conversion Solution] necessary for mounting, demounting, and removing adhesive from the wafer. In the 3M system, a glass plate (as shown in Fig. 3-23) is used to support the wafer through the back-grinding process. An ultraviolet (UV)–curable liquid adhesive is used as the bonding agent between the device wafer and the glass plate (support wafer). After the backgrinding process, as shown in Fig. 3-24, the thinned device wafer is transferred onto a dicing tape, and the support glass is removed by laser debonding of the adhesive-glass interface using a light-to-heat conversion (LTHC) layer. The adhesive then can be removed from the wafer, leaving behind fewer residues than seen with typical backgrinding tapes. This system also works for other semiconductor and packaging processes as long as the thermal-expansion mismatch between the device wafer and the glass plate is within the allowable tolerance.
3.4.2
EVG’s Temporary Bonding and Debonding System
EVG and Brewer Science have developed a solution that enables temporary bonding of a device wafer to a right carrier substrate (support wafer) and allows not only thinning but also a full range of subsequent
105
106
Chapter Three
Grinding stress to the wafer can be minimized because the UV-curable
Mount (spin coat UV resin on wafer; vacuum bond to support glass; UV irradiate)
adhesive flows into and supports the topography
Wafer
of the circuit patterns on
UV-cured liquid adhesive
the front side of the wafer.
LTHC layer
Support glass
The mounting process is
Because the wafer is fully
done under vacuum, ensuring that no bubbles
supported throughout
Back-grind
the back-grinding
are entrapped between
Grinding wheel
the wafer and the
process, less cracking is observed and higher
support glass.
yields can be obtained. Standard back-grinding
The laser debonding of
equipment is used; no
the adhesive-glass plate
significant back-grinding
interface is uniform, so
process changes are
no damage to the wafer
Laser irradiation
necessary. Laser
occurs when the glass plate is removed.
Dicing tape
Thinned wafer
Dicing
Remove support
Residue levels on the
Peel off UV resin layer
wafer surface after adhesive removal are lower than when using conventional back-grinding tapes.
FIGURE 3-24 3M wafer support system process flow (for wafer thinning).
processes, including high-temperature deposition, etching, lithography, dielectric application and curing, plating, and chemical cleaning, as shown in Fig. 3-25.36
Temporary Bonding The front side of the device wafer and the support wafer are coated with the WaferBOND, an HT Brewer Science adhesive material, by using the coating chamber (shown in Fig. 3-26) that includes spin and spray coat capability. Both wafers then are transferred to a bond
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Device wafer: Front-end processing (lithography, etching, etc.) Flip wafer Device wafer Carrier wafer with intermediate layer
TEMPORARY BONDING Device wafer bonded on carrier wafer
Back-thinning and further processing Device wafer (thin) on carrier wafer
DEBONDING
Cleaning
Thin-wafer handling Unloading in output format
FIGURE 3-25 EVG temporary bonding and debonding (of wafers) process flow.
chamber (EVG850TB), where they are carefully centered and vacuum bonded at elevated temperatures. Once the device wafer is temporarily bonded to the support wafer, it is ready for backside processing, including back-grinding, etching, metallization, TSV formation, etc.
Debonding During the debonding process, the thin wafer is debonded first via a thermally activated slide lift-off approach from the support wafer, cleaned in a single-wafer cleaning chamber to remove the remaining adhesive residues, and then transferred to the appropriate output format, such as a film-frame carrier, a dedicated wafer cassette, or a coin-stack packing canister, as shown in Figs. 3-25 and 3-27.
107
108
Chapter Three
FIGURE 3-26 EVG wafer-coating chamber, including spin and spray-coat capability.
The carrier wafer is also cleaned and then can be reused immediately for another debonding process.
3.4.3 A Simple Support-Wafer Method for Thin-Wafer Handling This section presents a very simple support-wafer method for thinwafer (50-μm) handling.32 The support-wafer fabrication process flow is shown in Fig. 3-28. The major process steps are photoresist (PR), lithography, release-hole etching using deep reactive-ion etch (DRIE), stripping of PR, and back-grinding to 500 μm. The device-wafer and perforated support-wafer bonding process flow is shown in
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
Thin-wafer cassette Megasonic
Processed device wafer
DI-water Solvent Diluted
Film frame
Chemistry Brush scrubber High pressure etc.
Carrier wafer
Coin stack
UV-exposure Single wafer carrier
DEBONDING
CLEANING
OUTPUT FORMAT
FIGURE 3-27 EVG debonding process flow, including debonding, cleaning, and outputting the thin wafer in various formats. Si wafer
Photoresist lithography
DRIE & stripping of PR
Back-grinding
Perforated support wafer
FIGURE 3-28 Support-wafer fabrication process flow.
Fig. 3-29 (left). The bonding adhesive used is the Waferbond from Brewer Science. The bonder used is the EVG bonder. The bonding parameters used are (1) 1.2 kN of applied force and (2) at 150ºC for 5 minutes. The wafer debonding process flow is shown in Fig. 3-29 (right). The major debonding steps are (1) soak in Waferbond remover solution at 90ºC and (2) remove wafer. The initial pitch between the two release holes on the perforated support wafer is 3.5 mm.
109
110
Chapter Three Wafer bonding
Wafer debonding
Device wafer Spin coating of adhesive Device wafer Support wafer
Wafer bonding
Device wafer Back-grinding to 50-μm
Stripping of adhesive Perforated support wafer (can be reused) + 50-μm-thick device wafer
FIGURE 3-29 Wafer bonding process flow (left) and wafer debonding process flow (right).
One of the key problems encountered in the support-wafer method is wafer debonding. The 50-μm-thick device wafer is easily broken during the wafer debonding process, as shown in Fig. 3-30. This key problem is resolved by optimizing the wafer debonding process to minimize residual stress. The first step is to reduce the pitch of the release hole on the perforated support wafer from 3.5 to 2 mm. The second step is to increase the number of perforations on the edge of the support wafer. These two optimized debonding methods allow more chemical solution to uniformly penetrate into the bonding adhesive and eventually debonded the wafers successfully, as shown in Fig. 3-31. Using the simple support-wafer method, thin-wafer transport and handling are possible. For example, the thin (50-μm) device wafer is attached to a support wafer and is handled and put in the PECVD FIGURE 3-30 Device wafer and perforated support wafer. 50-μm-thick device wafer
Perforated support wafer with 1-mm-diameter release holes
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g FIGURE 3-31 50-μm wafer after successful debonding.
50-μm-thick device wafer
Support wafer
50-μm-thick device wafer
FIGURE 3-32 The bonded perforated support wafer with the 50-μm device wafer in the plasma-therm chamber for the silicon dioxide PECVD process.
chamber for silicon dioxide deposition, as shown in Fig. 3-32. No wafer cracking is observed during wafer handling and after silicon oxide deposition. Thus thin-wafer handling using the support-wafer method is highly recommended. Some engineering and process development are required, though.
3.5
Low-Temperature Bonding for MEMS Packaging For 3D MEMS packaging, as mentioned in Chapter 2, the MEMS device/ wafer is bonded with the ASIC chip/wafer by either C2C or C2W bonding methods. Owing to chip yields and chip size differences, the W2W bonding method is seldom used. Most current bonding methods use temperatures higher than 300°C.37–39 During bonding, however, the
111
112
Chapter Three MEMS devices are already released (there are free-standing microstructures, e.g., membranes, beams, and cantilevers), and low-temperature bonding40–68 is desired to reduce damage to the microstructure owing to the thermal-expansion mismatch of the bonding structure (less bow). The bonding temperature for silicon C2C, C2W, and W2W bonding can be as low as RT40 (e.g., fusion bonding). However, for this kind of bonding, the bonding surfaces must be very flat and clean, which do not permit high-volume production, which is beyond the scope of this book. Low-melting solders such as In-Ag, In-Cu, In-Sn, In-Ni, and In-Sn-Cu, with bonding temperatures of less than 200°C, will be considered and presented in this and subsequent chapters.
3.5.1 How Does Low-Temperature Bonding with Solders Work? The basics of low-temperature bonding are shown in Figs. 3-33 and 3-34. It can be seen that the low-temperature solder (e.g., In-Ag, In-Cu, In-Sn, In-Ni, and In-Sn-Cu) is coated on the specially designed and Temperature, time, & pressure
Pick & place Micropads Micropads Low-melting solder
Micropads
Low-melting solder IMC
Low-melting solder Low-melting solder
Micropads
Micropads
Micropads
Aligning
Coating
Bond at 150–180°C, then all the interconnects become IMC with much higher remelt temperature
FIGURE 3-33 Fundamentals of low-temperature bonding. Wafer/Chip 2 Face UBM
Micropads
Face
Wafer/Chip 1
Transistor structure
Low-temperature solder
FIGURE 3-34 Face-to-face low-temperature bonding.
UBM
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g fabricated under-bump metallurgy (UBM). After aligning and bonding at a temperature of less than 200°C, all the solders will be reacted with the UBM (e.g., Cu, Cu/Au, and Cu/Ti/Au) of the pads (e.g., Al, Cu, Ni, Ag, and Au) on the chips/wafers and become an intermetallic compound (IMC) with a melting point that is (a couple of hundred degrees) higher than that of the solders. This feature is welcome by 3D MEMS packaging. For example, after the bonding of a MEMS device with an ASIC wafer with a lowmelting solder, all the bonding (solder-interconnect) areas become the IMC with a very high remelting temperature. When a cap wafer is bonded (with a low-temperature solder) to the ASIC wafer (already bonded with the MEMS device), the interconnect between the ASIC and the MEMS devices will not be reflowed. Furthermore, when the whole 3D MEMS package is attached to the PCB with surface-mounttechnology (SMT) lead-free solder (260°C), the solder interconnects between the ASIC and MEMS and cap and ASIC will not be reflowed.
3.5.2
Low-Temperature C2C Bonding
Figure 3-35 shows a schematic cross section of hermetic C2C lowtemperature bonding. The size of the bonding ring on the silicon base chip is 8 × 8 mm and the width of the bonding ring is 300 μm. The seed layers (SiO2, Si3N4, Ti, and Cu) and solder layers (In, Sn, and Au) are shown in the figure.42,43 The seed layers are fabricated by a sequential evaporation process along the bonding ring from a silicon wafer. This is followed by electroplating of the Cu and, finally, by E-beam
Cap Bonding ring
Base
SiO2 Si3N4
Silicon cap
Ti Cu
Au Sn
Silicon base
In Cu Ti Si3N4 SiO2
FIGURE 3-35 Schematic of a cap chip and a base chip with bonding ring (top) and their multilayer structures on the bonding ring.
113
114
Chapter Three sequential evaporation of the solder. The thickness of the Cu layer is 3 μm, the In layer is 1.6 μm, the Sn layer is 1.4 μm, and the Au layer is 50 nm. The very thin layer of Au is deposited on the Sn layer to inhibit oxygen penetration, which could happen when the samples are removed from the vacuum chamber and exposed to air. The silicon base-chip sizes are 10 × 10 mm. For the silicon cap chip, everything is the same except that there is no In, Sn, or Au. Figure 3-36 shows top and cross-sectional views of the as-received evaporated/electroplated bonding ring. It can be seen that the surface is very rough and has a granular structure with a grain size of 2 to 3 μm. In order to bond surfaces with such rough features, a molten solder layer and high pressure are necessary to fill the gaps between surfaces. Figure 3-37 shows the pull-test results (bond strength) of bonding couples under various bonding conditions (with the same bonding
In/Sn Cu Si
FIGURE 3-36 Scanning electron microscope (SEM) images of as-received evaporated composite coating surface (left) and its cross section (right). 8 5 minutes 20 minutes
Bonding strength, MPa
7 6 5 4 3 2 1 0
140
150
160 170 Temperature, °C
180
FIGURE 3-37 Effect of the bonding conditions on bonding strength.
190
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
FIGURE 3-38 Cross section of a bonding ring bonded at 1.5 MPa and 180°C for 20 minutes.
pressure of 1.5 MPa). It can be seen that higher bonding temperatures with longer bonding times yield better bond-strength results. Figure 3-38 shows a cross section of bonding couples obtained at 1.5-MPa bonding pressure and 180°C for 20 minutes. The thickness of the interconnect is uniform throughout the whole contact area with a typical value of 6.2 ± 0.5 μm. The bond couples are in good contact, and no interface line is observed, which means that the solder intermediate layers have melted during the bonding process and leveled the trough between granules. Acoustic images of the bond interface for chips bonded at 1.5 MPa of bonding pressure and 180°C for 20 minutes are shown in Fig. 3-39. The whole bonding ring is a uniform gray color, indicating that the bonded couples have intimate contact and that no voids or delamination occurred. The helium-leak-rate test results show that the bonding couples are hermetically sealed with an average leak rate of 5.8 × 10−9 (atm · ml)/s (the average of five samples). The fracture surfaces after pull tests are studied by x-ray diffraction (XRD) to examine the IMCs evolved in the bonding reaction zone. The AuIn2, Cu6Sn5, and Cu11In9 phases are found in the XRD analyses shown in Fig. 3-40. No peak of Sn or In is detected. Since the IMC layers are relatively thin, the transmission electron microscope (TEM) technique is used because it provides local chemical analysis. Figures 3-41 and 3-42, respectively, show TEM images of the region close to the base material silicon and interfacial reaction region between the Cu and solder intermediate layers. Figure 3-41 shows that on top of the silicon, the first layer is silicon oxide, followed by silicon nitride, titanium, and copper. The interfaces between each layer are void-free and uniform. The silicon oxide and nitride layers provide good adhesion between the subsequent metal layer and silicon base. Figure 3-42 shows the reaction zone between the Cu and Sn-In solder interlayer. Small grains are clearly visible in the reaction zone. The elemental composition results of the selected points are summarized
115
Chapter Three FIGURE 3-39 Acoustic images of a well-bonded flat silicon chip (left) and well-bonded patterned chips bonded at 1.5 MPa and 180°C for 20 minutes.
(a)
Bonding ring
(b)
800 ⊕
700
Δ
Δ
600 Intensity
116
⊗
Cu6Sn5 Cu11In9 AuIn2
500 400
⊗
300
100
⊗
Δ
Δ
Δ ⊕
Δ
0 25
⊕
Δ
Δ ⊕
200
30
35
40
45
50
⊗ Δ ⊕
55
⊗ ⊕
60 2θ
⊕Δ
⊗ Δ
65
⊕
70
FIGURE 3-40 XRD results of interface after pull tests.
⊗
75
⊕
⊕
80
⊗
85
⊗
90
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
Cu SiO2 & Si3N4
100 nm
Ti
Si
FIGURE 3-41 TEM image at the silicon region.
12 10 11 7 8 9 6 5 4
3
2 1 0.2 μm
FIGURE 3-42 TEM image at the interface region.
117
118
Chapter Three Composition (at percent) Point
Cu
In
Sn
Au
Phase
1
99.5
0.3
0.2
0
Cu
2
99
0.3
0.2
0.5
Cu
3
56.0
28.5
15.5
0
Cu11(In, Sn)9
4
54.6
31.3
13.7
0.4
Cu11(In, Sn)9
5
52.1
30.4
17.0
0.5
Cu11(In, Sn)9
6
51.4
28.3
19.6
0.7
Cu11(In, Sn)9
7
50.2
31.2
18.3
0.3
Cu11(In, Sn)9
8
48.1
21.0
30.4
0.5
η-Cu6(SnIn)5
9
49.8
23.4
26.6
0.2
η-Cu6(SnIn)5
10
50.3
20.7
29.0
0
η-Cu6(SnIn)5
11
5.9
59.0
1.1
34.0
Au(In, Sn)2
12
5.1
60.2
1.7
33.0
Au(In, Sn) 2
TABLE 3-7 Summary of Point EDX Analysis along the Interface Shown in the TEM Image
in Table 3-7. Two IMCs are identified along the main reaction zone, that is, Cu6(Sn, In)5 and Cu11(In, Sn)9. This result is very consistent with the XRD results, which confirmed the presence of these two IMCs in the bonding interface. The composition of Cu gradually reduces from 56 to 48 at percent from the near-Cu region to the near-In region. The energy dispersive x-ray (EDX) analysis suggests that there is still unreacted Cu that is not used for joint formation. At the edge of bonding interface, Cu composition drops dramatically, and only In and Au dominate, with the composition shown as points 11 and 12 in Table 3-7, that is, Cu5.9Au34In59.0Sn1.1 and Cu5.1Au33In60.2Sn1.7, which corresponds to an equilibrium-phase AuIn2. It is interesting to note that the overall composite solder is molten at 180°C, and the melting temperature of Sn is 230°C. This is so because the molten In layer is mixed with solid-state Sn layer and forms a thin, low-melting-temperature In-Sn layer at the interface. From the binary diagram, the eutectic In-Sn alloy has a lower melting point of 118°C, and at RT, the extent of Sn content in β phase ranges from 15 to 28 wt %, and the extent of In in γ phase can reach approximately 28 wt %. This means that In and Sn can easily diffuse into each other. Therefore, liquid In and solid Sn can interdiffuse into each other, and as a result, the eutectic In-Sn layer grows at the expense of the single In layer and Sn layer until both solder layers are completely consumed.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Notice that the initial overall composition of In and Sn present in the as-received base chip is the eutectic composition, that is, 48 wt % Sn. Although the In also reacts with Au, it consumes only a small portion of In, which leaves the overall In and Sn compositions slightly shifted to off-eutectic point, that is, with 50 wt % Sn. Thus, with such a near-eutectic liquid layer, the intrinsic roughness of the evaporated surface can be overcome, and a good joint interface is observed, as described earlier. During the soldering process, the subsequent interdiffusion of Cu and Sn or In takes place in the interface region and forms various IMCs. Because of the fully molten status of the intermediate layers at the temperature of 180°C, this may explain why the In atoms can interact with Au and form AuIn2 in the case where the Sn layer initially lies between the In layer and the Au. The composition analysis and XRD results also suggest that no unreacted In or Sn is present after bonding. The solder materials have completely transformed into IMCs by reacting with copper. This finding indicates that the bonding joint produced at low temperature can withstand high service temperatures owing to the presence of highmelting-point IMCs. From a consideration of the phase diagrams, the melting points of Cu6Sn5, Cu11In9, and AuIn2 are 430, 320, and 580°C, respectively. Therefore, the thermal stability of the joint is expected to be higher than 300°C. Figure 3-43 shows a slightly different solder system,50,51 where Cu/Au is used for the UBM, and the formation of mixed In-Cu and In-Au IMC phases are expected at the joint after bonding. The IMC phases and their melting temperatures could be checked in the phase diagrams (Fig. 3-44a and b). The structure and dimensions of various solder elements are shown in Fig. 3-43, where the bonding conditions, such as pressure (2.5 MPa), temperature (180°C), and time (20 minutes)
Si/SiO2 /Ti UBM (in μm)
Cu
Cu2Au0.03 Solder (in μm)
Sn
In
Sn
In
Au
Au
Sn0.5In2Sn0.5Au0.03
Bonding Parameters Temp Time Pressure (°C) (min) (MPa) 180
20
Cu Si/SiO2 /Ti
FIGURE 3-43 Schematic of the cap chip and base chip and their multilayer structures on the bonding ring.
2.5
119
Chapter Three 1200
1000 Liquid
Temperature, °C
800 FCC (Au) 600
Cu4In Cu7In3 Cu2In + Liquid
400
Cu11In9 + Liquid
Cu2In
200
Cu11In9
Cu11In9 + Tetragonal (In)
0 0
0.1
0.2
0.3
(a)
0.4 0.5 0.6 Mole fraction, In
0.7
0.8
0.9
1.0
1200
1000 Liquid 800
Temperature, °C
120
FCC (Au) 600 HCP_A3 400
AuIn_alpha1 AuIn3
AuIn2
Au7In2 200
Au3In
AuIn
Au7In3
AuIn2 + Tetragonal (In)
0 0 (b)
0.1
0.2
0.3
0.4 0.5 0.6 0.7 Weight fraction, In
0.8
0.9
FIGURE 3-44 (a) Phase diagram of Cu-In. (b) Phase diagram of Au-In.
1.0
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Cross-sectional SEM images
Heat flow, w/g
DSC curve showing remelting temperature > 400°C
ηCu6(InSn)5
–10
–15 0
100
200 300 Temperature, °C
400
500
FIGURE 3-45 Cross section of a joint bonded at 1.5 MPa and 180°C for 20 minutes (left) and its DSC curve (right).
are given. Figure 3-45 shows a void-free cross section and the differential scanning calorimetry (DSC) curve indicting that the remelting temperature is higher than 400°C. Figure 3-46 shows the very good helium-leakage test results and shear-strength test results. The lowtemperature interconnects also pass some reliability assessments, such as the pressure cook test (PCT), the high-temperature-storage test (HTS), and the thermal cycling test (TCT).
As Sealed
PCT
HTS
TCT
He leakage (atm · cc/s)
<5 × 10–8
<5 × 10–8
<5 × 10–8
<5 × 10–8
Shear strength (MPa)
27
34
28
18
8 mm
PCT: 121°C, 100%RH, 2 atm, 300 h HTS: 125°C, 1000 h TCT: –40/+125°C 1000 cycles
Seal ring
8 mm
FIGURE 3-46 Reliability assessment of C2C bonding with He leakage and shear strength tests.
121
122
Chapter Three
3.5.3
Low-Temperature C2W Bonding
Usually the chip size between MEMS and ASIC is not the same. Thus W2W bonding of these two devices may not be a good idea, and the interconnections generally are performed by either C2C or C2W bonding. This section discusses a MEMS chip with only the UBM bonded to an ASIC wafer with the low-temperature solders discussed in the preceding section. The ASIC wafer is shown in Figs. 3-47 and 3-48.
Alignment keys
Low-temp solder seal ring
Low-temp solder bonding pads AuInSn Ti/Cu/Au
ASIC wafer
FIGURE 3-47 Top and side views of an ASIC wafer with low-temperature solders. ASIC chip
FIGUSE 3-48 The fabricated ASIC wafer.
Seal ring
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Bonding and pickup tool MEMS chip
Low-temp solder
ASIC wafer
FIGURE 3-49 Pick and place the MEMS device on the ASIC wafer.
Both the bonding pads (for the MEMS device) and seal ring (for the cap wafer) are coated with low-temperature solders. Figures 3-49 and 3-50 show the MEMS chip being picked up and place on the ASIC wafer in an FC150 bonder. The bonding parameters are 6 MPa of bonding pressure at 200°C on the bonding tool (MEMS) and 90°C on the ASIC wafer, lasting for 40 seconds.50–53 The operation is performed in an enclosed N2 environment. Figure 3-51 shows a cross section of the bonding. There is no misalignment.
FIGURE 3-50 FC150 bonder (±1 μm) for C2W bonding.
123
124
Chapter Three
Shows good alignment
Bonding pad between MEMS device and ASIC wafer
FIGURE 3-51 Cross section of bonding between the MEMS device and the ASIC wafer.
3.5.4 Low-Temperature W2W Bonding An 8-in cap wafer is shown in Fig. 3-52. As mentioned earlier, its cavity is fabricated by the KOH etch process. The seal ring on the cap wafer is coated only with the UBM. Figure 3-53 shows a schematic of the cap wafer bonding to an ASIC wafer, which is accomplished in an EVG bonder with a pressure of 9 kN, temperature of 200°C, and bonding time of 20 minutes. 46–49 Figure 3-54 shows an x-ray
Cavity
Seal ring with UBM
FIGURE 3-52 The cap wafer with cavities and seal ring are coated with UBM only.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Cap wafer
ASIC wafer
FIGURE 3-53 Schematic of W2W bonding of a cap wafer and an ASIC wafer.
Bond pad (MEMS and ASIC)
Support wafer Seal ring
MEMS chip LT solder seal-ring bonding
X-ray picture of the bonded MEMS and ASIC wafers
LT solder bonding on 300-μm pads Bond pads between MEMS and ASIC (white arrows)
FIGURE 3-54 X-ray and SEM images indicate good alignment.
photograph and cross sections of the W2W bonding of the ASIC wafer and the cap wafer. It can be seen that (1) bond pads between the MEMS chip and the ASIC chip are in good alignment, and (2) there is no void in the solder sealing ring. Figure 3-55 shows the He leakage and shear strength test results. All the chips meet the specifications. After solder bumping and dicing, one of the individual packages is also shown in Fig. 3-55. It is ready to be put on a substrate in a package or on a PCB. It should be ensured that the bonding chamber for W2W bonding is free from debris. Because of the high vacuum during bonding, any particles present will cause the wafer to crack or form microcracks. Also, any significant misalignment between the ASIC wafer and the cap wafer could cause the entire wafer to be unusable. EVG’s SmartView Bond Aligner for face-to-face alignment can help. For more lowtemperature W2W bonding for 3D MEMS packaging, please see Chapter 4 and refs. 46 to 49.
125
126
Chapter Three Bond force
Temperature
Time
Shear strength (Cap-ASIC)
Shear strength (MEMS-ASIC)
Hermeticity (atmcc/sec)
9 kN
200°C
20 m
71.6 MPa
9.2 MPa
6 × 10–8
Completed package (face-to-face bonding) with solder ball attached
FIGURE 3-55 The completed package with solder ball attachment and reliability assessments.
3.6 MEMS Wafer Dicing Dicing of released MEMS wafers is not easy, especially for silicon-oninsulator (SOI) wafers and bonded wafers (e.g., silicon-on-silicon and silicon-on-glass) with etched patterns or circuitry. Compounded with very small MEMS die sizes and the requirement of very small street (kerf) widths (e.g., ≤100 μm) and chipping (e.g., ≤20 μm), dicing of MEMS wafers can be very challenging. Because of the exposed tiny/ thin, fragile, moving/pop-up structures (e.g., cantilevers, bridges, hinges, gears, and membranes), problems with stiction and debris are often encountered, thus decreasing manufacturing yields and increasing product costs. Use of the traditional diamond saw with water-jet cooling and cleaning is quite impossible without major modifications to the process steps. On the other hand, the stealth dicing (SD) technology uses a laser beam focused onto the MEMS silicon bulk and performs the internal transformation of silicon. The dies separate themselves by dicing-tape expansion, which effectively pulls the dies apart. This technology provides a dry, clean, nearly particle-free dicing process for sensitive MEMS devices. This section discusses dicing of SOI wafers and silicon-on-silicon bonded wafers using the SD method. Also, the dicing of silicon-on-glass bonded wafers is presented by the 2-step method developed by NEDO.
3.6.1
Fundamentals of SD Technology
Unlike the conventional laser dicing methods (i.e., laser ablation and laser breading),69–71 whose laser beam is focused on the wafer surface and the laser energy is absorbed on the wafer surface, the laser
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g FIGURE 3-56 Basic principles of SD technology.90–98
Laser
Focusing lens
SD layer
Si wafer
processing of SD method occurs only on the inside of the wafer; that is, the visible machining lines and the lines where cutting will be done remain hidden on the inside of the wafer, which is why the method is called stealth. There is little or no damage to the front and back sides of the wafer, as well as to the dicing tape on the backside of the wafer. The advantages of the SD method are (1) no chipping, (2) no debris contaminants, (3) a completely dry process, and (4) an environmentally friendly process. Figure 3-56 shows the basic principles of the SD technology72–77 developed by Hamamatsu Photonics. The laser beam is a 150-ns pulse Nd:YAG laser at a wavelength (>1000 nm, or 1064 nm) capable of transmitting through a silicon wafer that is condensed by an objective lens and focused onto a cleaving start point inside the wafer. By optimizing the laser and optical system to cause the absorption effect just in the vicinity of the focal point (also called the SD layer) inside the wafer, only localized points in the wafer can be selectively laser-machined without damaging the front and back surfaces of the wafer. The SD technology consists of two major processes. One is the laser process to form an SD layer (transformed area) on the interior of the wafer, and the other is the separation process to divide the wafer into small dies. Figure 3-57 (top) schematically shows the SD layer and the cracks that form on both sides of the SD layer, which extend toward (but do not reach) both surfaces of the wafer. Figure 3-57 (bottom) schematically shows wafer separation by tensile stresses induced by dicing-tape expansion. Figure 3-58 (top) shows the wafer before dicing-tape expansion, and Fig. 3-58 (bottom) shows the wafer after dicing-tape expansion, which is pushed up by a cylindrical stage. In this case, the 200-μm wafer is 50 μm thick, and individual die size is 10 × 10 mm.
127
128
Chapter Three
Cracks
Separated chip Tape expansion
Compression stress
Tensile stress
Tape expansion
FIGURE 3-57 SD technology: (top) laser transformation of silicon and (bottom) separation by tension.90–98
Chip
Wafer
Stage
Dicing tape Push up
FIGURE 3-58 Expansion process: (left) before expansion and (right) after tape expansion. When a cylindrical stage pushes up the dicing tape, the wafer on the dicing tape is separated into individual chips.90–98
For thicker silicon wafers, such as those with MEMS devices, in order to make it easier to separate the wafer into individual chips, the SD layers may have to be joined vertically while making multiple scans depth-wise in the wafer, as shown in Fig. 3-59. It can be seen in Fig. 3-59 (top) that the cracks have reached the laser irradiation surface, that is, the half-cut (HC), and Fig. 3-59 (middle) shows that the cracks have reached laser irradiation bottom surface, that is, the bottomside half-cut (BHC). Figure 3-59 (bottom) shows crack propagation of the BHC case under tape expansion. Owing to the stress concentration at the crack tip, the wafer is easily separated into individual dies.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g Wafer
Crack extension Tensile stress
Tape expansion
Cracks
Wafer
Tape Tape expansion
BHC
Crack extension Tensile stress Tape Tape expansion
Tape expansion
Crack has reached upper surface Wafer
Cracks
Tensile stress
Tape expansion
Tape
Tape expansion
FIGURE 3-59 Fundamental principles of crack extension.90–98
Figure 3-60 shows SEM images of a MEMS sensor device (2 × 2 × 300 mm) with a membrane structure that has been diced by the SD method. A hollow with a depth of several microns is constructed in the center of the chip, and the actual sensor device is formed on the opposite side of the chip. It can be seen that (1) there is no chipping, (2) there are sharp and clean dicing lines, and (3) there is no trace of damage or debris. Figure 3-61 shows the sidewalls of a MEMS sensor chip (after SD laser processing and tape expansion) provided by the Fraunhofer Institute78 on the European Downscaled Assembly of Vertically Interconnected Devices (DAVID) project. Again, it can be seen that (1) no material abrasion or ablation has occurred; (2) the method minimizes the contamination risk on the die surface; and (3) the method completely avoids edge chipping.
3.6.2
Dicing of SOI Wafers
Figure 3-62 shows the results of dicing wafers with a SOI layer by the SD method.69–77 One of the unique features of today’s SOI wafers is that they have a buried silicon oxide (buried oxide or box) layer extending across the entire wafer. By optimizing the laser and optical system, SD layers can be formed in the SOI layer, box layer, and silicon layer, as shown in Fig. 3-62 for a MEMS sensor wafer. It can be seen from the SEM images that the wafer is (1) chip-free, (2) dust-particle-free, (3) with sharp surfaces, and (4) without damage to the fragile structure.
129
130
Chapter Three
1000 μm
100 μm
FIGURE 3-60 SEM images of chip cut with SD technology.90–98
3.6.3
Dicing of Silicon-on-Silicon Wafers
Figure 3-63 shows photographs and an SEM image of a diced silicon-onsilicon bonded wafer separated by the SD method. Similar results to those with SOI wafers have been achieved. DISCO has developed a new laser machine (DFL7340/7360) that uses the SD technology developed by Hamamatsu Photonics as a dicing solution for MEMS wafers and thin wafers.69–77
3.6.4
Dicing of Silicon-on-Glass Wafers
For silicon-on-glass wafers, it is very difficult to form the SD layer (internal transformation) inside the glass wafer with the laser. A new MEMS dicing method for glass wafers has been reported by the MEMS
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
50 μm
500 × 20 mm 21.8.08 9:20:41 10 kV
FIGURE 3-61 SEM image of a MEMS chip after stealth dicing.99
SOl layer Box layer
Laser 50 μm
Box layer
Si layer
25 μm
SOl layer cross section
SOI layer
85 μm 3 μm
SOl layer surface quality
500 μm Tape expansion
Si layer 100 μm
No damage to sensor
50 μm
Wafer cross section
SEM image
FIGURE 3-62 SOI wafer diced by SD technology.90–98
131
132
Chapter Three SiO2
SiO2
.5 μm
Si layer SiO2
300 μm .5 μm 300 μm
Si layer
SiO2
50 μm SiO2 layer surface quality
FIGURE 3-63 Dicing of silicon-on-silicon wafers with the SD technology.90–98
project from the New Energy and Industrial Technology Development Organization (NEDO) of Japan.79 There are two process steps. The first is to form the international transformation, and the second is to separate the wafer by a CO2 laser–induced thermal stress. Unlike the SD method, whose internal transformation of silicon is based on the thermal effect of single-photon absorption, the new method’s internal transformation of glass is based on multiphoton absorption and thus a shorter-pulse-width (10 ns and 100 fs) laser with a high peak intensity. For separation of a glass wafer into individual chips, a 25-W CO2 laser with a wavelength of 10.6 μm is used, and the laser radiation is absorbed by the SiO2 and suitable for a local heat source in the glass. Figure 3-64a shows the dicing results of a silicon (300 μm) on Pyrex-glass
Glass/Si (3 mm × 3 mm)
Internal modification 100 μm
FIGURE 3-64 Dicing of a silicon-on-glass wafer.100
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g (300 μm) bonded wafer, and Fig. 3-64b shows a MEMS package consisting of a (100-μm-thick) silicon and (500-μm-thick) Pyrex-glass wafer. It can be seen that (1) the dicing lines follow the internal transformation, (2) the edges are sharp, (3) it is chip-free, and (4) neither debris nor damage is found. It should be pointed out that the contamination on the surface is formed during the MEMS processing and is not due to the dicing.
3.7
RoHS-Compliant MEMS Packaging In this section, the EU RoHS directive will be presented first. It should be emphasized that the information provided herein is intended to be of assistance to exporters who ship their products with MEMS devices and packages anywhere in the world, especially EU countries. While every effort has been taken to ensure the accuracy of the information presented here, given the dynamic nature of such information, special attention should be paid to the latest announcements/publications by the governments of the EU countries and especially the EU Commission. The impacts of RoHS, such as lead-free-solder joint reliability, on MEMS packaging will be presented later.
3.7.1 EU RoHS Since February 13, 2003, the Restriction of the Use of Certain Hazardous Substances (RoHS) directive has been law in the European Union (EU),80 and it was implemented on July 1, 2006. It bans lead (Pb), mercury (Hg), cadmium (Cd), hexavalent chromium (Cr6+), and two types of brominated flame retardants, polybrominated biphenyls (PBBs) and polybrominated diphenyl ethers (PBDEs). This means that all electrical and electronic equipment (EEE), except those with exemptions,80–88 cannot be put on the EU market if they contain any of those six banned materials. A list of products (the categories of EEE) that covered by the EU RoHS directive is shown in the Annex of Waste Electrical and Electronic Equipment (WEEE) directive.89 1. Large household appliances 2. Small household appliances 3. Information technology and telecommunications equipment 4. Consumer equipment 5. Lighting equipment 6. Electrical and electronic tools (with the exception of largescale stationary industrial tools) 7. Toys and leisure and sports equipment 10. Automatic dispensers It should be pointed out that as of today, category 8 (i.e., medical devices, with the exception of all implanted and infected products)
133
134
Chapter Three and category 9 (i.e., monitoring and control instruments), which covered by the WEEE directive, are not covered by the RoHS directive.
3.7.2 What Is the Definition of X-Free (e.g., Pb-Free)? The maximum concentration value (MCV) of those six banned materials permitted in “homogeneous materials” of EEEs has been published in the Official Journal of the EU and become a law on August 18, 2005.90 The journal stated: “For the purposes of Article 5(1)(a), a MCV of 0.1 percent by weight in homogeneous materials for lead, mercury, hexavalent chromium, polybrominated biphenyls (PBBs), and polybrominated diphenyl ethers (PBDEs) and of 0.01 percent by weight in homogeneous materials for cadmium shall be tolerated.” In plain language, lead-free is defined as a content of lead in all (individual) homogeneous materials of an EEE that is less than 0.1 wt %.
3.7.3 What Is a Homogeneous Material? According to the EU Commission’s guidance, homogeneous materials are as follows.91 1. Homogeneous material means a material that cannot be mechanically disjointed into different materials. 2. The term homogeneous means “of uniform composition throughout.” Examples of homogeneous materials include individual types of plastics, ceramics, glass, metals, alloys, paper, board, resins, and coatings. 3. The term mechanically disjointed means that the materials can, in principle, be separated by mechanical actions such as unscrewing, cutting, crushing, grinding, and abrasive processes. Some EU Commission examples of the application of this guidance91 include 1. A plastic cover is a homogeneous material if it consisted exclusively of one type of plastic that was not coated with or has attached to it or inside it any other kinds of materials. In this case, the MCV of the RoHS directive would apply to the plastic. 2. An electrical cable that consisted of metal wires surrounded by nonmetallic insulation materials is an example of a nonhomogeneous material because the different materials could be separated by mechanical processes. In this case, the MCV of the RoHS directive would apply to each of the separated materials individually. 3. A semiconductor package contains many homogeneous materials, which include the plastic molding material, the tinelectroplating coatings on the lead frame, the lead-frame alloy, and the gold-bonding wires.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
3.7.4 What Is the TAC? There are 27 members of the Technical Adaptation Committee (TAC) of the EU. Each member represents her or his own member state (country). They have the utmost power because their role is to provide technical changes and exemptions, as well as interpretation of the EU RoHS directive. (Thus, if you are not clear about some specific MEMS packaging issue of a product to be shipped into a particular country, you can ask a TAC member, and the contact information for each is listed on his or her country’s Web site.) TAC members report to the EU Commissioner. All of them receive the same information from the Commissioner, but they don’t have the same voting power. The votes from some member states (e.g., the United Kingdom and Germany) will carry more weight than that of others (e.g., Greece and Ireland).
3.7.5
How Is a Law Published in the EU RoHS Directive?
After the TAC’s yes vote on an item (usually exemption), the EU Commissioner will consult with the Parliament and Council. If the Parliament agrees, then the Commissioner will sign the ruling and publish it in the Official Journal of the EU, and it becomes a law.
3.7.6
EU RoHS Exemptions
One of the key implementation methods of the EU RoHS directive is by exemptions,80–88 which many thousands of products have relied on (i.e., exemption from the RoHS directive). Companies from all over the world are entitled to apply for exemptions as long as they have enough supporting data. With the recommendations of consultants such as ERA Technology (in the United Kingdom) and the Oko Institute (in Germany), the TAC will vote on the exemptions and report the voting result to the EU Commissioner. At present, there are 32 exemptions, and they are as follows: 1. Mercury in compact fluorescent lamps not exceeding 5 mg per lamp 2. Mercury in straight fluorescent lamps for general purposes not exceeding halophosphate, 10 mg; triphosphate with normal lifetime, 5 mg; and triphosphate with long lifetime, 8 mg 3. Mercury in straight fluorescent lamps for special purposes 4. Mercury in other lamps not specifically mentioned in this Annex 5. Lead in glass of cathode-ray tubes, electronic components, and fluorescent tubes 6. Lead as an alloying element in steel containing up to 0.35 percent lead by weight, aluminium containing up to 0.4 percent lead by weight, and as a copper alloy containing up to 4 percent lead by weight
135
136
Chapter Three 7. Lead in high-melting-temperature solders (i.e., lead-based alloys containing 85 percent by weight or more lead); lead in solders for servers; storage and storage array systems; and network infrastructure equipment for switching, signaling, transmission, and network management for telecommunications; lead in electronic ceramic parts (e.g., piezoelectronic devices) 8. Cadmium and its compounds in electrical contacts and cadmium plating, except for applications banned under Directive 91/338/EEC amending Directive 76/769/EEC relating to restrictions on the marketing and use of certain dangerous substances and preparations 9. Hexavalent chromium as an anticorrosion agent for carbon steel cooling systems in absorption refrigerators a. Deca-BDE in polymeric applications b. Lead in lead-bronze bearing shells and bushes 10. Within the procedure referred to in Article 7(2), the Commission shall evaluate the applications for: Deca-BDE; mercury in straight fluorescent lamps for special purposes; lead in solders for servers, storage and storage array systems, network infrastructure equipment for switching, signaling, transmission, and network management for telecommunications (with a view to setting a specific time limit for this exemption), and light bulbs as a matter of priority in order to establish as soon as possible whether these items are to be amended accordingly 11. Lead used in compliant pin connector systems 12. Lead as a coating material for a thermal conduction module C-ring 13. Lead and cadmium in optical and filter glass 14. Lead in solders consisting of more than two elements for connection between the pins and the package of microprocessors with a lead content of more than 80 percent and less than 85 percent by weight 15. Lead in solders to complete a viable electrical connection between semiconductor die and carrier within integratedcircuit flip-chip packages 16. Lead in linear incandescent lamps with silicate-coated tubes 17. Lead halide as radiant agent in high-density discharge (HID) lamps used for professional reprography applications 18. Lead as an activator in the fluorescent powder (1 percent lead by weight or less) of discharge lamps when used as tanning
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g lamps containing phosphors such as BaSi2O5:Pb (BSP), as well as when used as specialty lamps for diazoprinting reprography, lithography, insect traps, and photochemical and curing processes containing phosphors such as (Sr, Ba)2MgSi2O7: Pb (SMS) 19. Lead with PbBiSn-Hg and PbInSn-Hg in specific compositions as the main amalgam and with PbSn-Hg as an auxiliary amalgam in very compact energy saving lamps (ESLs) 20. Lead oxide in glass used for bonding front and rear substrates of flat fluorescent lamps used for liquid-crystal displays (LCDs) 21. Lead and cadmium in printing inks for the application of enamels on borosilicate glass 22. Lead as impurity in rare earth iron-garnet (RIG) Faraday rotators used for fiberoptic communications systems 23. Lead in finishes of fine-pitch components other than connectors with a pitch of 0.65 mm or less with NiFe lead frames and lead in finishes of fine-pitch components other than connectors with a pitch of 0.65 mm or less with copper lead frames 24. Lead in solders for the soldering of machined through-hole discoidal and planar array ceramic multilayer capacitors 25. Lead oxide in plasma display panels (PDPs) and surfaceconduction electron emitter displays (SEDs) used in structural elements, notably in the front and rear glass dielectric layer, the bus electrode, the black stripe, the address electrode, the barrier ribs, the seal frit and frit ring, and print pastes 26. Lead oxide in the glass envelope of black-light-blue (BLB) lamps 27. Lead alloys as solder for transducers used in high-powered (designated to operate for several hours at acoustic power levels of 125 dB SPL and above) loudspeakers 28. Hexavalent chromium in corrosion-preventive coatings of unpainted metal sheetings and fasteners used for corrosion protection and electromagnetic interface shielding in equipment falling under category 3 of Directive 2002/96/EC (IT and telecommunications equipment) (Exemption granted until 1 July 2007.) 29. Lead bound in crystal glass as defined in Annex I (categories 1, 2, 3, and 4) of Council Directive 69/493/EEC 30. Cadmium alloys as electrical/mechanical solder joints to electrical conductors located directly on the voice coil in transducers used in high-powered loudspeakers with sound pressure levels of 100 dB(A) and more
137
138
Chapter Three 31. Lead in soldering materials in mercury-free flat fluorescent lamps (which, for example, are used for LCDs and design or industrial lighting) 32. Lead oxide in seal frits used for making window assemblies for argon and krypton laser tubes
3.7.7 Current Status of RoHS Compliance in the Electronics Industry Since 2000, the electronics industry has spent billions of dollars on compliance with the RoHS directive. More than 95 percent of the effort has been directed at eliminating lead (Pb), that is, creating lead-free materials, developing soldering process, performing characterization measurements, and reliability assessments, etc. The eutectic SnPb solder (63 wt % Sn and 37 wt % Pb), with a melting point of 183°C, has been the predominant choice for assembling electronics products for decades owing to its outstanding solderability and reliability. Unfortunately, because of the RoHS directive, Pb is banned in most electronics products that include MEMS components/modules. Not long ago, there were more than 100 lead-free solder alloys to be chosen from, as shown in Table 3.1 of ref. 92. However, because of the very tight regulatory deadlines, the industry has “rushed” to select SnAgCu solder alloys and is “in a great hurry” to build the infrastructure around the Sn(1 to 4 wt %)Ag(0.5 to 0.7 wt %)Cu lead-free solder family. The melting point of these solders is around 217°C, which is 34°C higher than that of SnPb solder. Thus, during assembly, the components (including MEMS) and PCBs will be subjected to higher soldering temperatures, and their cost, performance, and reliability are of great concern to manufacturers.92–129 Higher energy consumption is another concern.98 Owing to a lack of experimental and simulation data, one of the critical issues of lead-free soldering is solder-joint reliability, especially for high-reliability (>10 years of life) products. As discussed earlier, MEMS packaging consists of solder materials for sealing, die attachment, solder bumps, and/or solder balls. Thus the solder-joint reliability of MEMS packages is under scrutiny.
3.7.8
Lead-Free Solder-Joint Reliability of MEMS Packages
A number of environmental stress factors [e.g., temperature, voltage, humidity, corrosion, current density (electromigration), and mechanical loads) may lead to MEMS lead-free solder sealing-ring and/or solder-joint failure. The most commonly failure modes in practice are overload and fatigue.97,119 Overload failure occurs whenever the stress in a MEMS solder joint, brought about by the imposed stress factors, is greater than the capacity of the solder material. An example would be excessive bending and twisting of a PCB with a solder-bumped ASIC/MEMS chip
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g or PBGA package housing a MEMS device soldered to its surface. In this case, the bending and twisting stresses are larger than the strength or fracture toughness of the lead-free solder material. Fatigue failure takes place via the initiation and propagation of a crack until it becomes unstable. The stress factors that typically cause failure by fatigue are far below the overload failure levels. Examples of fatigue failure include the temperature cycling and/or vibration of a solder-bumped chip, chip scale package (CSP), or ball grid array (BGA) package that is soldered to the surface a PCB. This section will consider both the temperature and drop fatigue stress factors.
Definition of Reliability Reliability of a solder joint of a particular package (e.g., MEMS) in electronic products is defined as the probability that the solder joint will perform its intended function for a specified period of time under given operating conditions without failure.97,119 Numerically, reliability is the percent of survivors; that is, R(t) = 1 – F(t), where R(t) is the reliability (survival) function and F(t) is the cumulative distribution function (CDF). Life distribution is a theoretical population model used to describe the lifetime of a solder joint and is defined as the CDF, that is, F(t), for the solder-joint population. Thus the one and only way to determine solder-joint reliability is by reliability testing.
Objective of Reliability Tests The objective of reliability tests is to obtain failures (the more the better) and to best fit the failure data to (determine the parameters of) the CDF of a chosen probability distribution (e.g., Weibull). The number of items (i.e., sample size) to be tested should be such that the final data are statistically significant. The reliability test time is unknown but usually takes a while (e.g., a few months). It should be noted and emphasized that as soon as the life distribution F(t) of the lead-free solder joint of a particular package with a certain chip size is estimated by reliability testing, the reliability R(t), failure rate, cumulative failure rate, average failure rate, mean time to failure, etc. of the lead-free solder joints are readily determined.97 Most reliability tests are accelerated tests (with increased intensity of exposure to aggressive environmental conditions and realistic sample sizes and test times). Thus acceleration models are needed to transfer the failure probability, reliability function, failure rate, and mean time to failure from a test condition to an operating condition. In establishing the acceleration models for lead-free solder joints, their surrounding materials (e.g., solder, molding plastic, ceramic, copper, fiber-reinforced glass epoxy, and silicon), loadings (e.g., stress, strain, temperature, humidity, current density, and voltage), and failure mechanisms and modes (e.g., overload, fatigue, corrosion, and electromigration) must be considered.
139
140
Chapter Three
Reliability Test Methods Some common tests for solder joints include • Temperature cycling tests (e.g., –40 to 125°C) • Power cycling tests (depends on devices) • Functional cycling tests (depends on devices) • High/low-temperature storage tests (120°C/–20°C) • Biased 85/85 tests (e.g., 85°C/85 %RH, 1.8 V) • High-voltage extended-life tests (e.g., 100°C, 1.8 V) • Pressure-cook tests (autoclave tests) (e.g., 121°C, 2 atm) • Salt-atmosphere tests (MIL-STD-883D) • Moisture-sensitivity tests (e.g., IPC/JEDEC-020C) • Shock (drop) tests (e.g., 1.3- to 1.5-mm drops) • Vibration tests (e.g., random vibration) • Mechanical bending, shearing, and twisting tests (e.g., IPC/ JEDEC-9702) • Electromigration tests (e.g., see ref. 129) • Others For solder-joint reliability, most of these tests, in general, are very expensive and time-consuming. Thus, before and after reliability testing, design for reliability (DFR) and failure analysis (FA) have been very useful and important tools for solder-joint reliability.
Reliability Engineering of Solder joints Figure 3-65 shows the concept of reliability engineering of solder joints.97,119 It consists of three major tasks, namely, DFR, reliability testing and data analysis, and FA. Usually, the procedure starts with a design of the solder joints of a MEMS package with the given MEMS device size and package, the solder alloys, and the corresponding PCB and demonstrates that the design is electrically, thermally, and mechanically sound. As an example, the DFR activity is often performed with a finite-element simulation using the material properties of all the structural elements and the imposed boundary conditions. The next step in the process is for a certain number of samples of the sound or reliable design to be built and tested under certain conditions for a certain period of time. The test data (failures) then are analyzed and fitted into a life-distribution (or reliability) designation for the solder joints. Failure analysis (FA) then should be done on the failed samples to find out the root cause and understand the reason for their failure. This information is very useful for
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
• Eliminate trial-anderror of reliability tests • Reduce cost • Reduce design/test/FA cycles
• Provide insight into the physical, chemical, electrical, mechanical, and thermal behaviors of the structure • Provide failure locations, failure modes, and failure mechanisms
Design for reliability
• Sample size
• Verify the reliability test data
• Test condition
Reliability engineering
• Test period • Obtain failures • Life distribution
Reliability test & data analysis
• Verify the DFR analysis results Failure analysis
• Reliability function • Failure rate • Mean time to failure
• Understand why it failed and how to fix it or do better for the next round of DRF and reliability test • Choose acceleration models to determine the acceleration factors
FIGURE 3-65 Reliability engineering.
1. Providing the failure locations, failure modes, and failure mechanisms 2. Verifying the reliability-test data 3. Verifying the DFR simulation results 4. Understanding why the sample failed and how to fix it (or to do better) 5. The next round of DFR and reliability testing 6. Choosing acceleration models to determine the acceleration factors because most of the reliability tests are naturally “accelerated” Some common methods for solder-joint FA are • Visual inspection • X-ray inspection • A-, B-, and C-mode scanning acoustic microscopy (SAM) • Dye and pry • Cross-sectioning • High-power microscopy • Scanning electron microscopy (SEM) • Focused ion beam (FIB) and SEM
141
142
Chapter Three • X-ray diffraction (XRD) • Transmission electron microscopy (TEM) • Energy-dispersive x-ray spectrometry (EDX) • Tomographic acoustic microimaging (TAMI) • Others It should be noted and emphasized that the reliability obtained from DFR is not the same as the reliability (probability) obtained from reliability tests. For example, the life (number of cycles to failure) of a solder joint from reliability tests depends on the percent failed (or survived). Statistically, there are an infinite number of possible lives; for example, the characteristic life corresponds to 63.2 percent failed (or 36.8 percent survived). On the other hand, the best we can do from DFR is to predict a (one) life of the solder joint for a given boundary condition. As another example, the failure rate (i.e., the number of solder joints that failed in the first year, second, third, etc. year) can be determined from the reliability test. However, the DFR does not even know what failure rate means. In the past 2 decades, with the advancement of computers, DFR of solder joints has become as important as the reliability test. Even though it cannot predict solder-joint reliability, failure rate, mean time to failure, etc., DFR is usually performed by a mathematical modeling based on the material properties of the structure and laws of engineering and physics in order to 1. Eliminate trial-and-error reliability tests 2. Reduce cost 3. Reduce design/test/FA cycles 4. Reduce time to market 5. Provide insight into the physical, chemical, electrical, mechanical, and thermal behaviors of solder joints (e.g., the maximum stress/strain locations) to help test-board designs to capture the most likely (solder-joint) failure locations and to help FA to find these failures sites
Material Properties of Lead-Free Solders for MEMS Packaging In order to perform DFR and fully understand the engineering physics of solder-joint reliability, the material properties of solders must be known (through tests) and understood. Some important material properties of solders are • Phase-transition temperatures (i.e., solidus, liquidus, plastic, and eutectic) • Melting point
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g • Boiling point • Softening point • Hardness • Density • Dispensability • Glass-transition temperature • Coefficient of thermal expansion • Vapor pressure • Surface tension • Storage modulus • Loss modulus • Viscosity • Miscibility • Electrical conductivity • Thermal conductivity • Stress-strain curves • Shear strength • Tensile strength • Ultimate strength • Elongation • Yield strength • Young’s modulus • Poisson’s ratio • Creep curves • Stress-relaxation curves • Creep rates • Creep rupture • Fracture toughness • Viscoelasticity • Viscoplasticity • Fatigue strength • Isothermal fatigue curves • Fatigue crack-growth curves • Moisture absorption • Others
143
Young’s modulus, GPa
Chapter Three 60 95.5Sn-3.9Ag-0.6Cu 40 SnPb
20
0 0
50
100
150
200
Temperature, °C
FIGURE 3-66 Young’s modulus of lead-free and tin-lead solders.
For example, the Young’s modulus of the lead-free (SAC) and tin-lead (Sn-Pb) solder alloys is shown in Fig. 3-66.109 The figure shows that the modulus of the lead-free solder alloy is larger than that of the Sn-Pb solder alloy. Therefore, for a given structural geometry and boundary condition, one should expect higher stresses in the leadfree solder joints compared with the Sn-Pb eutectic solder joints. For another example, the creep responses of SAC and Sn-Pb solders at 50°C are presented in Fig. 3-67.110 The figure shows that the Sn-Pb solder has a creep rate that is greater than that of the SAC solder. As a result, for a given structural geometry and boundary condition, the Sn-Pb solder joints should have both a faster creep response and higher creep strains. The cost, performance, quality, and reliability of solder joints will be affected by the preceding materials properties (>35) of the solder that forms the joints. However, it should be reemphasized that the reliability of solder joints cannot be determined by the materials properties of the solder but rather by reliability tests.
Tensile creep strain rate, 1/s
144
1.0E-04 1.0E-05 1.0E-06 1.0E-07 1.0E-08 1.0E-09 1.0E-10 1.0E-11 1.0E-12 1.0E-13
50°C
Sn-Pb SAC 1
10 Tensile stress, MPa
100
FIGURE 3-67 Tensile creep-strain rate for SAC and Sn-Pb solder alloys at 50°C.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g 1200 1064.43
1000
Lower-melting point (217°C) eutectic Au90wt%Sn. Flux is needed unless use expansive process, e.g., pressure, plasma, …
Liquid 800 °C
600
Au
Fluxless Au20wt%Sn (280°C) eutectic
532
519
419.3
400 ζ
β
280°C
276 29 190
200
72
309 50.5
252
18.5
231.97 η
217
93.7 βSn
10
0
δ
ζ’
13 ε
αSn
–200 0 Au
10
20
30
40 50 60 Atomic percent, Sn
70
80
90
100 Sn
FIGURE 3-68 Au-Sn solder phase diagram.
AuSn for MEMS Packaging Au-Sn solders are especially suited for MEMS packaging. Most of the MEMS devices have to be soldered in a fluxless process, which is possible using Au-Sn solders, as shown in the phase diagram in Fig. 3-68. Also, most of the manufacturing processes for the cap wafer and the ASIC wafer already include Au plating, which makes the use of Au-Sn solders attractive. Furthermore, 80 wt % Au–20 wt % Sn solder is used widely because of its advantages, namely, high strength, high corrosion resistance, and high fatigue resistance. Thus the Au20Sn solder system is usually selected as the sealing material for MEMS (cap-waferto-ASIC-wafer bonding) applications.
Au-Sn Solder Lift-Off Process Au-Sn solder can be manufactured by various methods, such as evaporation, electrodeposition, paste and solder preform. Among these methods, evaporated solder allows more accurate control of dimensions and positions. Therefore, after under-bump metallurgy (UBM) patterning, a sequence of Sn-Au layers (in total, eight layers of Sn and eight layers of Au) is evaporated and simultaneously patterned by a lift-off process. The thickness of each Sn and Au layer is 0.2 and 0.24 μm, respectively. The evaporation is done in a Temescal E-Beam Evaporator (Model VES-2550) from Semicore Equipment, Inc. The evaporation rate is 5 Å/s. During the lift-off process, a 20-μm-thick dry film is used as a mold.
145
146
Chapter Three
W2W Au-Sn Solder Bonding After the formation of all the solder layers, wafer-level bonding is conducted to bond the cap wafer and the ASIC wafer. The bonding is carried out at 350°C with a 15-minute dwell at peak temperature and a compressive pressure of 4.7 MPa. After bonding, the W2W-bonded wafer is diced into individual stacks for shear testing, which shows that the shear strength of the bonding is higher than 27.2 MPa. (In this case, the spec is 6 MPa.) Of course, the W2W bonding also can be performed with low-temperature solders, as mentioned in Sec. 2.5.4.
Quality of Lead-Free Solder Joints During lead-free process development and manufacturing, the following tests usually are performed: • Wetting balance test • Solder-spreading test • Solderability test • Cleanability test • Printability test • Temperature-profiling test • Surface-insulation-resistance (SIR) test • Automated optical inspection (AOI) test • X-ray inspection test • In-circuit test (ICT) • Functional test • Shear test • Pull test • Bend tests • Others These tests are very useful for developing the assembly process and for improving manufacturing yield. Thus these tests will enhance and ensure the quality of the solder joints. However, these tests cannot determine solder-joint reliability, which has to be obtained by reliability tests.
Reliability Test of Lead-Free MEMS PBGA Solder Joints Figure 3-69 shows a very typical Weibull probability plot from the thermal-cycling reliability test results of Sn3Ag0.5Cu (SAC) lead-free solder joints. In this case, it is for a 256-pin plastic ball-grid array (PBGA) package as shown in Figs. 2-45, 2-46, and 2-47 in Chapter 2. It can be seen that for the test samples, at 2000 cycles (–25 to 125°C, one cycle per hour), 6 percent of the PBGA solder joints have failed, and 94 percent have survived, that is, the reliability is 0.94.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g 90.00 Sample size = 20
50.00
Percent failed, F (x)
Median rank No. of failures = 16
10.00 5.00
Weibull slope β = 2.8 1.00 Characteristic life θ = 5466 cycles
0.50 β1 = 2.7750, η1 = 5465.7692, ρ = 0.9936
0.10 1500.00
John Lau Agilent
6000.00 Cycles to failure (x)
FIGURE 3-69 Thermal-cycling test of lead-free 256-pin PBGA package on a PCB (–25 to 125°C, one cycle per hour).
Figure 3-70 shows the life distribution of the lead-free PBGA at 90 percent confidence. At 90 percent confidence for a given 256-pin PBGA lead-free solder joint, that is, in 90 of 100 cases, the true characteristic life θt of the 256-pin PBGA lead-free solder joint will happen within the interval 4480 ≤ θt ≤ 6021 cycles. At the same time, it can be shown that the true mean life (which occurs at 51 percent failed) μ of the PBGA lead-free solder joints, in 90 of 100 cases (i.e., at 90 percent confidence), can be as low as 3822 cycles and as high as 4865 cycles, that is, 3822 ≤ μ ≤ 4865 cycles. The higher the required confidences, the wider are the life intervals. From solder-joint-uniformity points of view, for example, the true Weibull slope can be estimated from determination of the Weibull slope error E, which depends on the number of failures N and the required confidence C, as reported in refs. 100, 117, 119, 120, and 122. For example, in the present case, there are 16 failures (N = 16), and the required confidence is 90 percent (C = 0.9); then E = 30 percent.100,117,119,120,122 Thus the true Weibull slope βt of the 256-pin PBGA lead-free solder joint can be at least 1.95 but not more than 3.61, that is, 1.95 ≤ βt ≤ 3.61. Now you have done your reliability tests and data analysis properly and have obtained the life distribution, reliability function, failure rate, mean time to failure, etc., so what? How do you apply these test results to your products under operating conditions? What are the acceleration factors of lead-free solder joints under, for example, thermal, mechanical, shock and vibration, electromigration, and corrosion
147
Chapter Three 90.00 Sample size = 20
50.00 95% rank Percent failed, F (x)
148
No. of failures = 16
10.00 Sample weibull Slope β = 2.8
5.00 50% rank
5% rank Sample Characteristic life θ = 5466 cycles
1.00 0.50 β1 = 2.7750, η1 = 5465.7692, ρ = 0.9936 β2 = 4.1568, η2 = 6020.5530, ρ = 0.9908 β3 = 2.0446, η3 = 4480.3343, ρ = 0.9830
0.10 1500.00
John Lau Agilent
6000.00 Cycles to failure, (x)
FIGURE 3-70 Lead-free 256-pin PBGA with 90 percent confidence (–25 to 125°C, 1-hour thermal cycle).
conditions? What are the field failure data of lead-free solder joints to verify the acceleration models? The industry is still working very hard in these areas. In many situations, the qualities and uniformities of two products (e.g., two sets of solder joints) are to be compared based on knowledge of limited test data. One of the difficult tasks in reliability life testing is to draw conclusions about a population from a small sample size, as shown in preceding sections. It is even more difficult to compare the populations of two sets of solder joints (e.g., lead-free and tin-lead) based on knowledge of their limited test data. If one set of solder joints is found to be superior to another, how confident can one be that the same is true of their populations? (A simple equation reported in refs. 100, 117, 119, 120, and 122 can be used to determine this confidence, which is not the same as the required confidence discussed in preceding sections.) Now you have done the reliability tests of lead-free and tin-lead solder joints under the same test conditions and have determined that one is better than the other with very high confidence, so what? How do you know that it is also true at operating considerations such as thermal, mechanical, electromigration, corrosion, humidity, current density, shock, and vibration conditions? Again, the industry is still working very hard in these areas. Maybe another $5 billion of efforts will do it!
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g
References 1. Andry, P. S., Tsang, C. K., Webb, B. C., Sprogis, E. J., Wright, S. L., Bang, B., and Manzer, D. G. “Fabrication and characterization of robust through-silicon vias for silicon-carrier applications.” IBM Journal of Research and Development 52:571–581, 2008. 2. Knickerbocker, J. U., Andry, P. S., Dang, B., Horton, R. R., Patel, C S., Polastre, R. J., Sakuma, K., Sprogis, E. S., Tsang, C. K., Webb, B. C., and Wright, S. L. “3-D silicon integration.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 538–543. 3. Kumagai, K., Yoneda, Y, Izumino, H., Shimojo, H., Sunohara, M., and Kurihara, T. “A silicon interposer BGA package with Cu-filled TSV and multi-layer Cu-plating interconnection.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 571–576. 4. Sunohara, M., Tokunaga, T., Kurihara, T., and Higashi, M. “Silicon interposer with TSVs (through silicon vias) and fine multilayer wiring.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 847–852. 5. Lee, H. S., Choi, Y.-S., Song, E., Choi, K., Cho, T., and Kang, S. “Power delivery network design for 3D SIP integrated over silicon interposer platform.” In IEEE Proceedings of Electronic Components and Technology Conference, Reno, NV, May 2007, pp. 1193–1198. 6. Ramm, P., Wolf, M., Klumpp, A., Wieland, R., Wunderle, B., Michel, B., and Reichl, H. “Through silicon via technology: Processes and reliability for wafer-level 3D system integration.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 847–852. 7. Matsuo, M., Hayasaka, N., and Okumura, K. “Silicon interposer technology for high-density package.” In IEEE Proceedings of Electronic Components and Technology Conference, Las Vegas, NV, May 2000, pp. 1455–1459. 8. Wright, S., Andry, P. S., Sprogis, E., Dang, B., and Polastre, R. J. “Reliability testing of through-silicon vias for high-current 3D applications.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 879–883. 9. Selvanayagam, C., Lau, J. H., Zhang, X., Seah, S., Vaidyanathan, K., and Chai, T. “Nonlinear thermal stress/strain analysis of copper filled TSV (through silicon via) and their flip-chip microbumps.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 1073–1081. 10. Wong, E., Minz, J., and Lim, S. K. “Effective thermal via and decoupling capacitor insertion for 3D system-on-package.” in IEEE Proceedings of Electronic Components and Technology Conference, San Siego, CA, May 2006, pp. 1795–1801. 11. Yu, A., Khan, N., Archit, G., Pinjalal, D., Toh, K., Kripesh, V., Yoon, S., and Lau, J. H. “Development of silicon carriers with embedded thermal solutions for high power 3-D package.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 24–28. 12. Beica, R., Sharbono, C., and Ritzdorf, T. “Through silicon via copper electrodeposition for 3D integration.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 577–583. 13. Premachandran, C. S., Lau, J. H., Ling, X., Khairyanto, A., Chen, K., and Myo Ei Pa Pa. “A novel, wafer-level stacking method for low-chip yield and non-uniform, chip-size wafers for MEMS and 3D SIP applications.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 314–318. 14. Zhang, X., Chai, T., Lau, J. H., Selvanayagam, C., Biswas, K., Liu, S., Pinjala, D., Tang, G., Ong, Y., Vempati, S., Wai, E., Li, H., Liao, B., Ranganathan, N., Kripesh, V., Sun, J., Doricko, J., and Vath, C. “Development of through silicon via (TSV) interposer technology for large die (21 × 21 mm) fine-pitch Cu/low-k FCBGA package.” In IEEE Electronic Components and Technology Conference, San Diego, CA, May 2009, pp. 305–312.
149
150
Chapter Three 15. Wolf, M., Wunderle, B., Jürgensen, N., Engelmann, G., Ehrmann, O., Michel, B., Dretschkow, T., Uhlig, A., and Reichl, H. “High aspect ratio TSV copper filling with different seed layers.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 563–570. 16. Khan, N., Rao, V., Lim, S., Ho, S., Lee, V., Zhang, X., Yang, R., Liao, E., Ranganathan, T., Chai, T., Kripesh, V., and Lau, J. H. “Development of 3D silicon module with TSV for system in packaging.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 550–555. 17. Ho, S., Yoon, S., Zhou, Q., Pasad, K., Kripesh, V., and Lau, J. H. “High rf performance TSV for silicon carrier for high frequency application.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 1956–1952. 18. Ranganathan, N., Ebin, L., Linn, L., Lee, V., Navas, O., Kripesh, V., and Balasubramanian, N. “Integration of high aspect ratio tapered silicon via for through-silicon interconnection.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 859–865. 19. Henry, D., Jacquet, F., Neyret, M., Baillin, X., Enot, T., Lapras, V., BrunetManquat, C., Charbonnier, J., Aventurier, B., and Sillon, N. “Through silicon vias technology for CMOS image sensors packaging.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 556–562. 20. Chen, K., Premachandran, C., Choi, K., Ong, C., Ling, X., Khairyanto, A., Ratmin, B., Myo, P., and Lau, J. H. “C2W bonding method for MEMS applications.” In IEEE Proceedings of Electronic Packaging Technology Conference, Singapore, December 2008, pp. 1283–1287. 21. Sunohara, M., Tokunaga, T., Kurihara, T., and Higashi, M. “Silicon interposer with TSVs (through silicon vias) and fine multilayer wiring.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 2008, pp. 847–852. 22. Miura, H., Nishimura, A., Kawai, S., and Murakami, G. “Structural effect of IC plastic package on residual stress in silicon chips.” In IEEE Proceedings of Electronic Components and Technology Conference, Las Vegas, NV, May 20–23, 1990, pp. 316–32. 23. Sweet, J. N. “Die stress measurement using piezoresistive stress sensor.” In Thermal Stress and Strain in Microelectronics Packaging, edited by J. H. Lau, pp. 221–268. New York: Van Nostrand Reinhold, 1993. 24. Rahim, M., Suhling, J. C., Copeland, D. S., Islam, M. S., Jaeger, R. C., Lall, P., and Johnson, R. W. “Die stress characterization in flip-chip on laminate assemblies.” IEEE Trans. Comp. Packag. Technol. 28:415–429, 2005. 25. Bittle, D., Suhling, J. C., Beaty, E. E., Jaeger, R. C., and Johnson, R. W. “Piezoresistive stress sensors for structural analysis of electronic packages.” J. Electron. Packag. 113:203–210, 1991. 26. Lo, T., and Chan, P. C. H. “Design and calibration of a 3-D micro-strain gauge for in-situ on chip stress measurements.” In Proceedings of the ICSE, Malaysia, November 1996, pp. 252–255. 27. Gee, S., Akylas, V. R., and Bogert, W. F. “The design and caliberation of a semiconductor strain gauge array.” Proc. IEEE Microelectron. Test Structure 1:185–191, 1988. 28. Zhong, Z., Zhang, X., Sim, B. H., Wong, E. H., Teo, P. S., and Iyer, M. K. “Caliberation of a piezoresistive stress sensor in (100) silicon test chips.” In Proceedings of the IEEE Electronic Packaging Technology Conference, Singapore, December 8–11, 2002, pp. 1–4. 29. Beaty, R., Jaeger, R. C., Suhling, J. C., Johnson, R. W., and Butler, R. D. “Evalution of piezoresistive coefficient variation in silicon stress sensor using a four-point bending test fixture.” IEEE Trans. Comp. Hybrids Manufact. Technol. 15:904–914, 1992. 30. Suhling, J., Cordes, R. A., Kang, Y. L., and Jaeger, R. C. “Wafer-level caliberation of stress sensing test chips.” In IEEE Proceedings of Electronic Components and Technology Conference, Washington DC, May 1–4, 1994, pp. 1058–1070.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g 31. Slattery, O., Mahoney, D. O., Sheehan, E., and Waldron, F. “Source of variation in piezoresistive stress sensor measurements.” IEEE Trans. Comp. Packag. Technol. 27:81–86, 2004. 32. Zhang, X., Kumar, A., Zhang, Q., Ong, Y., Ho, D., Khong, C., Kripesh, V., Lau, J., Kwong, D., Sundaram, V., and Tummula, R. “Application of piezoresistive stress sensors in ultra thin device handling and characterization.” In Proceedings of Eurosensors Conference, Dresden, Germany, September 7–10, 2008, pp. 1022–1026. 33. Suhling, J., and Jaeger, R. C. “Silicon piezoresistive stress sensors and their applications in electronic packaging.” IEEE Sensors J. 1:14–30, 2001. 34. Kumar, A., Zhang, X., Zhang, Q., Jong, M., Huang, G., Kripesh, V., Lee, C., Lau, J., Kwong, D., Sundaram, V., Tummula, R., and Meyer-Berg, G. “Evaluation of stresses in thin device wafer using piezoresistive stress sensor.” In IEEE Proceedings of Electronic Packaging and Technology Conference, Singapore, December 9–12, 2008, pp. 1270–1276. 35. www.3m.com/electronicmaterial. 36. Pargfrieder, S., Kettner, P., Privett, M., and Ting, J. “Temporary bonding and debonding enabling TSV formation and 3D integration for ultra-thin wafers.” In Proceedings of the 10th IEEE Electronics Packaging Technology Conference, Singapore, December 2008, pp. 1301–1305. 37. Klumpp, A. “Vertical system integration by using inter-chip vias and solidliquid interdiffusion bonding.” Jpn. J. Appl. Phys. 43:L829–L830, 2004. 38. Chen, K. “Microstructure examination of copper wafer bonding.” J. Electron. Mater. 30:331–335, 2001. 39. Morrow, P. R. “Three-dimensional wafer stacking via Cu-Cu bonding integrated with 65-nm strained-Si/low-k CMOS technology.” IEEE Electron. Device Lett. 27:335–337, 2006. 40. Shimbo, M., Furukawa, K., Fukuda, K., and Tanzawa, K. “Silicon-to-silicon direct bonding method.” J. Appl. Phys. 60:2987–2989, 1986. 41. Made, R., Gan, C. L., Yan, L., Yu, A.,Yoon, S. U., Lau, J. H., and Lee, C. “Study of low temperature thermocompression bonding in Ag-In solder for packaging applications.” J. Electron. Mater. 38:365–371, 2009. 42. Yan, L.-L., Lee, C.-K., Yu, D.-Q., Yu, A.-B., Choi, W.-K., Lau, J. H., and Yoon, S.-U. “A hermetic seal using composite thin solder In/Sn as intermediate layer and its interdiffusion reaction with Cu.” J. Electron. Mater. 38:200–207, 2009. 43. Yan, L.-L., Lee, V., Yu, D.,Choi, W. K., Yu, A.,Yoon, S.-U., and Lau, J. H. “A hermetic chip to chip bonding at low temperature with Cu/In/Sn/Cu joint.” In IEEE Proceedings of Electronics and Components Technology Conference, Orlando, FL, May 2008, pp. 1844–1848. 44. Yu, A., Lee, C., Yan, L., Made, R., Gan, C., Zhang, Q., Yoon, S., and Lau, J. H. “Development of wafer level packaged scanning micromirrors.” Proc. Photon. West 6887:1–9, 2008. 45. Lee, C., Yu, A., Yan, L., Wang, H., Han, J., Zhang, Q., and Lau, J. H. “Characterization of intermediate In/Ag layers of low temperature fluxless solder based wafer bonding for MEMS packaging.” J. Sensors Actuators (in press). 46. Yu, D.-Q., Lee, C., Yan, L. L., Choi, W. K., Yu, A., and Lau, J. H. “The role of Ni buffer layer on high yield low temperature hermetic wafer bonding using In/Sn/Cu metallization.” Appl. Phys. Lett. (in press). 47. Yu, D. Q., Yan, L. L., Lee, C., Choi, W. K., Yoon, S. U., and Lau, J. H. “Study on high yield wafer to wafer bonding using In/Sn and Cu metallization.” In Proceedings of the Eurosensors Conference, Dresden, Germany, 2008, pp. 1242–1245. 48. Yu, D., Lee, C., and Lau, J. H. “The role of Ni buffer layer between InSn solder and Cu metallization for hermetic wafer bonding.” In Proceedings of the International Conference on Electronics Materials and Packaging, Taipei, Taiwan, October 22–24, 2008, pp. 335–338.
151
152
Chapter Three 49. Yu, D., Yan, L., Lee, C., Choi, W., Thew, M., Foo, C., and Lau, J. H. “Wafer level hermetic bonding using Sn/In and Cu/Ti/Au metallization.” In IEEE Proceeding of Electronics Packaging and Technology Conference, Singapore, December 2008, pp. 1–6. 50. Choi, W., Yu, D., Lee, C., Yan, L., Yu, A., Yoon, S., Lau, J. H., Cho, M., Jo, Y., and Lee, H. “Development of low temperature bonding using In-based solders.” In IEEE Proceedings of Electronics Component and Technology Conference, Orlando, FL, May 2008, pp. 1294–1299. 51. Choi, W., Premachandran, C., Ong, C., Ling, X., Liao, E., Khairyanto, A., Chen, K., Thaw, P., and Lau, J. H. “Development of novel intermetallic joints using thin film indium based solder by low temperature bonding technology for 3D IC stacking.” In IEEE Proceedings of Electronics Component and Technology Conference, San Diego, CA, May 2009, pp. 333–338. 52. Chen, K., Premachandran, C., Choi, K., Ong, C., Ling, X., Khairyanto, A., Ratmin, B., Myo, P., and Lau, J. H. “C2W bonding method for MEMS applications.” In IEEE Proceedings of Electronics Packaging Technology Conference, Singapore, December 2008, pp. 1283–1287. 53. Premachandran, C. S., Lau, J. H., Ling, X., Khairyanto, A., Chen, K., and Myo Ei Pa Pa. “A novel, wafer-level stacking method for low-chip yield and non-uniform, chip-size wafers for MEMS and 3D SIP applications.” In IEEE Proceedings of Electronic Components and Technology Conference, Orlando, FL, May 27–30, 2008, pp. 314–318. 54. Simic, V., and Marinkovic, Z. “Room temperature interactions in Ag-metals thin film couples.” Thin Solid Films 61:149–160, 1979. 55. Lin, J.-C. “Solid-liquid interdiffusion bonding between In-coated silver thick films.” Thin Solid Films 61:212–221, 1979. 56. Roy, R., and Sen, S. K. “The kinetics of formation of intermetallics in Ag/In thin film couples.” Thin Solid Films 61:303–318, 1979. 57. Chuang, R. W., and Lee, C. C. “Silver-indium joints produced at low temperature for high temperature devices.” IEEE Trans. Components Packag. Technol. A 25:453–458, 2002. 58. Chuang, R. W., and Lee, C. C. “High-temperature non-eutectic indium-tin joints fabricated by a fluxless process.” Thin Solid Films 414:175–179, 2002. 59. Lee, C. C., and Chuang, R. W. “Fluxless non-eutectic joints fabricated using gold-tin multilayer composite.” IEEE Trans. Components Packag. Technol. A 26:416–422, 2003. 60. Humpston, G., and Jacobson, D. Principles of Soldering and Brazing, pp 128–132. Materials Park, MD: ASM International, 1993. 61. Chuang, T., Lin, H., and Tsao, C. “Intermetallic compounds formed during diffusion soldering of Au/Cu/Al2O3 and Cu/Ti/Si with Sn/In interlayer.” J. Electron. Mater. 35:1566–1570, 2006. 62. Lee, C., and Choe, S. “Fluxless In-Sn bonding process at 140°C.” Mater. Sci. Eng. A333:45–50, 2002. 63. Lee, C. “Wafer bonding by low-temperature soldering.” Sensors & Actuators 85:330–334, 2000. 64. Vianco, P. T. “Intermetallic compound layer formation beteween copper and hot-dipped 100 In, 50In-50Sn, 100Sn and 63Sn-37Pb coatings.” J. Electron. Mater. 23:583–594, 1994. 65. Frear, D. R. “Intermetallic growth and mechanical-behavior of low and highmelting temperature solder alloys.” Metall. Mater. Trans. A 25:1509–1523, 1994. 66. Morris, J. W. “Microstructure and mechancial property of Sn-In and Sn-Bi solders.” J. Miner. Metals Mater. Soc. 45:25–27, 1993. 67. Mei, Z. “Superplastic creep of low melting-point solder joints.” J. Electron. Mater. 21:401–407, 1992. 68. Chuang, T. H. “Phase identification and growth kinetics of the intermetallic compounds formed during In-49Sn/Cu soldering reactions.” J. Electron. Mater. 31:640–645, 2002.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g 69. Hermanns, C. “Laser separation of flat glass.” In Proceedings of 63th Laser Materials Processing Conference, Miami, FL, October 31–November 3, 2005, pp. 105–109. 70. Richerzhagen, B., Perrottet, D., and Kozuki, Y. “Dicing of wafers by patented water-jet-guided laser: The total damage-free cut.” In Proceedings of 65th Laser Materials Processing Conference, Kyoto, Japan, May 16–19, 2006, pp. 197–200. 71. Chall, P. “ALSI’s low power multiple beam technology for high throughput and low damage wafer dicing.” In Proceedings of 65th Laser Materials Processing Conference, Kyoto, Japan, May 16–19, 2006, pp. 211–215. 72. Kumagai, M., Uchiyama, N., Ohmura, E., Sugiura, R., Atsumi, K., and Fukumitsu, K. “Advanced dicing technology for semiconductor wafer: Stealth dicing.” IEEE Trans. Semiconduct. Manufact. 20:259–265, 2007. 73. Monodane, T., and Ohmura, E. “Thermo-elastic-plastic analysis on intenal processing phenomena of single-crystal silicon by nanosecond laser.” In Proceedings of 65th Laser Materials Processing Conference, Kyoto, Japan, May 16–19, 2006, p. 06-125. 74. Fukuyo, F., Fukumitsu, K., and Uchiyama, N. “Stealth dicing technology and applications.” In Proceedings of 6th International Symposium on Laser Precision Microfabrication, Williamsburg, VA, April 4–8, 2005. 75. Fukumitsu, K., Kumagai, M., Ohmura, E., Morita, H., Atsumi, K., and Uchiyama, N. “The mechanism of semiconductor wafer dicing by stealth dicing technology.” In Proceedings of 4th International Congress Laser Advanced Materials Processing, Scottsdale, AZ, October 30–November 2, 2006. 76. Ohmura, E., Fukuyo, F., Fukumitsu, K., and Morita, H. “Internal modifiedlayer formation mechanism into silicon with nano second laser.” J. Achiev. Mater. Manufact. Eng. 17:381–384, 2006. 77. Ohmura, E., Fukumitsu, K., Uchiyama, N., Atsumi, K., Kumagai, M., and Morita, H. “Analysis of modified layer formation into silicon wafer by permeable nanosecond laser.” In Proceedings of the International Congress of Applications Lasers and Electro-Optics, Scottsdale, AZ, October 30–November 2, 2006, pp. 24–31. 78. Marenco, N., Reinert, W., Warnat, S., Lange, P., Gruenzig, S., Hillmann, G., Kostner, H., Bock, G., Guadagnuolo, S., and Conte, A. “Vacuum encapsulation of resonant MEMS sensors by direct chip-to-wafer stacking on ASIC.” In IEEE Proceedings of Electronics Packaging and Technology Conference, Singapore, December 9–12, 2008, pp. 773–777. 79. Izawa, Y., Tanaka, S., Kikuchi, H., Tsurumi, Y., Miyanago, N., Esashi, M., and Fujita, M. “Debris-free in-air laser dicing for multi-layer MEMS by perforated internal transformation and thermally-induced crack propagation.” In IEEE Proceeding of MEMS, Tucson, AZ, January 13–17, 2008, pp. 822–827. 80. The European Parliament and the Council of the European Union, “Directive 2002/95/EC on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, February 13, 2003, pp. L 37/19–23. 81. Commission Decision. “Amending Directive 2002/95/EC of the European Parliament and of the Council for the Purpose of Establishing the Maximum Concentration Values for Certain Hazardous Substances in Electrical and Electronic Equipment (EEE).” Official J. European Union, August 19, 2005, p. L 214/65. 82. Commission Decision. “Amending for the Purposes of Adapting to the Technical Progress the Annex to Directive 2002/95/EC of the European Parliament and of the Council on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, October 15, 2005, pp. L 271/48–50. 83. Commission Decision. “Amending for the Purposes of Adapting to the Technical Progress the Annex to Directive 2002/95/EC of the European Parliament and of the Council on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, October 25, 2005, pp. L 280/18–19.
153
154
Chapter Three 84. Commission Decision. “Amending for the Purposes of Adapting to the Technical Progress the Annex to Directive 2002/95/EC of the European Parliament and of the Council on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, April 28, 2006, pp. L 115/38–39. 85. Commission Decision. “Amending for the Purposes of Adapting to the Technical Progress the Annex to Directive 2002/95/EC of the European Parliament and of the Council on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, October 14, 2006, p. L 283/47. 86. Commission Decision. “Amending for the Purposes of Adapting to the Technical Progress the Annex to Directive 2002/95/EC of the European Parliament and of the Council on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, October 14, 2006, p. L 283/48. 87. Commission Decision. “Amending for the Purposes of Adapting to the Technical Progress the Annex to Directive 2002/95/EC of the European Parliament and of the Council on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, October 14, 2006, pp. L 283/50–51. 88. Commission Decision. “Amending for the Purposes of Adapting to the Technical Progress the Annex to Directive 2002/95/EC of the European Parliament and of the Council on the Restriction of the Use of Certain Hazardous Substances (RoHS) in Electrical and Electronic Equipment (EEE).” Official J. European Union, May 24, 2008, pp. L 136/9–10. 89. European Parliament and Council of the European Union. “Directive 2002/96/EC on Waste Electrical and Electronic Equipment (WEEE).” Official J. European Union, February 13, 2003, pp. L 37/24–38. 90. Commission Decision. “Amending Directive 2002/95/EC of the European Parliament and of the Council for the Purpose of Establishing the Maximum Concentration Values for Certain Hazardous Substances in Electrical and Electronic Equipment (EEE).” Official J. European Union, August 19, 2005, p. L 214/65. 91. TAC Report. “RoHS Enforcement Guidance Document,” Version 1, UK, May 2006, pp. 13–14. 92. Lau, J. H. Low-Cost Flip Chip Technologies for DCA, WLCSP, and PBGA Assemblies. New York: McGraw-Hill, 2000. 93. Lau, J. H., Wong, C. P., Prince, J. L., and Nakayama, W. Electronic Packaging: Design, Materials, Process, and Reliability. New York: McGraw-Hill, 1998. 94. Lau, J. H., and Lee, R. Chip Scale Package. New York: McGraw-Hill, 1999. 95. Lau, J. H., and Lee, R. Microvias for Low Cost, High Density Interconnects. New York: McGraw-Hill, 2001. 96. Lau, J. H., Wong, C. P., Lee, N. C., and Lee, R. Electronics Manufacturing with Lead-Free, Halogen-Free, and Conductive Adhesive Materials. New York: McGraw-Hill, 2003. 97. Lau, J. H., and Pao, Y. H. Solder Joint Reliability of BGA, CSP, Flip Chip, and Fine Pitch SMT Assemblies. New York: McGraw-Hill, 1997. 98. Geiger, D., Shangguan, D., and Yi, S. “Thermal study of lead-free reflow soldering processes.” In Proceedings of the 3rd IPC/JEDEC Annual Conference on Lead-Free Electronic Assemblies and Components, San Jose, CA, 2003, pp. 95–98. 99. Lau, J. H., Harkins, G., Rice, D., Kral, J., and Wills, B. “Experimental and statistical analysis of surface-mount technology PLCC solder-joint reliability.” IEEE Transactions of Reliability 37:524–530, 1988. 100. Lau, J. H. “Reliability Testing and Data Analysis,” workshop at the NEPCON West, Anaheim, CA, February 1990. 101. Tu, K. N. “Recent advances on electromigration in very-large-scale-integration of interconnects.” J. Appl. Phys. 94:5451–5473, 2003.
E n a b l i n g Te c h n o l o g i e s f o r A d v a n c e d M E M S P a c k a g i n g 102. Lau, J. H., Mei, Z., Pang, S., Amsden, C., Rayner, J., and Pan, S. “Creep analysis and thermal-fatigue life prediction of the lead-free solder sealing ring of a photonic switch.” ASME Trans. J. Electron. Packag. 124:403–410, 2002. 103. Lau, J. H., and Lee, R. “Modeling and analysis of 96.5Sn-3.5Ag lead-free solder joints of wafer level chip scale package (WLCSP) on “build-up microvia printed circuit board.” IEEE Trans. Electron. Packag. Manufact. 25:51–58, 2002. 104. Lau, J., Dauksher, W., Smetana, J., Horsley, R., Shangguan, D, Castello, T., Menis, I., Love, D., and Sullivan, B. “Design for lead-free solder joint reliability of high-density packages.” J. Solder. Surface Mount Technol. 16:12–26, 2004. 105. Lau, J. H., and Dauksher, W. “Reliability of an 1657CCGA (ceramic column grid array) package with 96.5Sn3.9Ag0.6Cu lead-free solder paste on PCBs (printed circuit boards).” ASME Trans. Electron. Packag. 127:96–105, 2005. 106. Lau, J., Hoo, N., Horsley, R., Smetana, J., Shangguan, D., Dauksher, W., Love, D., Menis, I., and Sullivan, B. “Reliability testing and data analysis of leadfree solder joints for high-density packages.” J. Solder. Surface Mount Technol. 16:46–68, 2004. 107. Lau, J., Shangguan, D., Castello, T., Horsley, R., Smetana, J., Dauksher, W., Love, D., Menis, I., and Sullivan, B. “Failure analysis of lead-free solder joints for high-density packages.” J. Solder. Surface Mount Technol. 16:69–76, 2004. 108. Lau, J. H. “Impacts of RoHS (e.g., Pb-Free) on Electronic Products,” workshop at the IPC/JEDEC 9th International Conference on Lead-Free Electronic Components and Assemblies, Singapore, August 17, 2005. 109. Lau, J. H., Dauksher, W., and Vianco, P. “Acceleration models, constitutive equations and reliability of lead-free solders and joints.” In IEEE Electronic Components and Technology Conference Proceedings, New Orleans, LA, June 2003, pp. 229–236. 110. Lau, J. H., and Dauksher, W. “Creep constitutive equations of Sn(3.5–3.9)wt %Ag(0.5–0.8)wt %Cu.” In Micromaterials and Nanomaterials, edited by B. Michel, pp. 54–62. Berlin: Fraunhofer Institute IZM, 2004. 111. Lau, J. H., Lee, R., Dauksher, W., Shangguan, D., Song, F., and Lau, D. “A systematic approach for determining the thermal fatigue-life of plastic ball grid array (PBGA) lead-free solder joints.” ASME Paper No. IPACK200573364, New York, July 2005. 112. Lau, J. H., Goh, S., Tay, G., Erasmus, S., Sporon-Fiedler, F., and Pan, S. “Characterization of bump chip carrier (BCC++) package assembly and solder joint reliability for fiber-optic transceiver applications.” IEEE Trans. Components Packag. Technol. 2009. 113. Lau, J. H., Lo, J., Lam, J., Soon, E., Chow, W., and Lee, R. “Effects of underfills on the thermal-cycling tests of SnAgCu PBGA (plastic ball grid array) packages on ImAg PCB (printed circuit board).”IEEE Trans. Adv. Packag. (in press). 114. Lau, J. H. “Thermal stress analysis of a flip-chip parallel VCSEL (verticalcavity surface-emitting laser) package with low-temperature lead-free (48Sn-52In) solder joints.” IEEE Trans. Adv. Packag. (in press). 115. Lau, J. H., Pang, J., Lee, N., and Xu, L. “Material properties and intermetallic compounds of a new lead-free solder: Sn3wt %Ag0.5wt %Cu0.019wt %Ce (SACC).” IEEE Trans. Adv. Packag. (in press). 116. Lau, J. H., Gleason, J., Schroeder, V., Henshall, G., Dauksher, W., and Sullivan, B. “Design, materials, and assembly process of high-density packages with a low-temperature lead-free solder (SnBiAg).” Solder. Surface Mount Technol. 20:11–20, 2008. 117. Lau, J. H., Gleason, J., Schroeder, V., Henshall, G., Dauksher, W., and Sullivan, B. “Reliability test and failure analysis of high-density packages assembled with a low-temperature lead-free solder (SnBiAg).” Solder. Surface Mount Technol. 20:21–29, 2008. 118. Lau, J. H., Castello, T., Shangguan, D., Dauksher, W., Smetana, J., Horsley, R., Love, D., Menis, I., and Sullivan, R. “Failure analysis of lead-free solder joints of an 1657CCGA (ceramic column grid array) package.” J. Microelectron. Electron. Packag. 4:189–213, 2007.
155
156
Chapter Three 119. Lau, J. H. “Reliability of lead-free solder joints.” ASME Trans. Electron. Packag. 128:297–301, 2006. 120. Lau, J., and Dauksher, W. “Reliability of an 1657CCGA (ceramic column grid array) package with 96.5Sn3.9Ag0.6Cu lead-free solder pasties on PCBs (printed circuit boards). ASME Trans. Electron. Packag. 127:96–105, 2005. 121. Lau, J., Dauksher, W., Smetana, J., Horsley, R., Shangguan, D., Castello, T., Menis, I., Love, D., and Sullivan, B. “Design for lead-free solder joint reliability of high-density packages.” J. Solder. Surface Mount Technol. 16:12–26, 2004. 122. Lau, J. H., Tse, P., Richard, E., Dauksher, W., Shangguan, D., Pang, J. “Reliability of Sn3wt %Ag0.5wt %Cu0.019wt %Ce (SACC) solder joints.” In IEEE Electronic Components and Technology Conference Proceedings, San Diego, CA, May 2009, pp. 415–422. 123. Lau, J. H., Pang, J., Lee, N.-C., and Xu, L. ”Material properties and intermetallic compounds of a new lead-free solder: Sn3wt %Ag0.5wt %Cu0.019wt %Ce (SACC).” In IEEE Proceedings of Electronic Components and Technology Conference, Reno, NV, May 29–June 1, 2007, pp. 211–218. 124. Lau, J. H., Liu, S., Shangguan, D., Song, Z., and Geiger, D. “Process development and solder joint reliability of a new lead-free solder: Sn3wt %Ag0.5wt %Cu0.019wt %Ce (SACC).” In IEEE Proceedings of Electronics Packaging Technology Conference, Singapore, December 10–12, 2007, pp. 546–552. 125. Lau, J. H., Shangguan, D., Lau, D., Kung, T., and Lee, R. “Thermal-Fatigue Equation for Wafer-Level Chip Scale Package (WLCSP) Lead-Free Solder on Lead-Free Printed Circuit Board (PCB).” In IEEE Proceedings of Electronic Components and Technology Conference, Las Vegas, NV, June 1–4, 2004, pp. 1563–1569. 126. Lau, J. H., and Dauksher, W. “Thermal stress analysis of a flip-chip parallel VCSEL (vertical-cavity surface-emitting laser) package with low-temperature lead-free (48Sn-52In) solder joints.” In IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 30–June 2, 2006, pp. 1009–1017. 127. Lau, J. H., Lee, R., Song, F., Lau, D., and Shangguan, D. “Isothermal fatigue tests of plastic ball grid array (PBGA) SnAgCu lead-free solder joints at 60°C.” In IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 30–June 2, 2006, pp. 1476–1483. 128. Lau, J. H., and Dauksher, W. “Effects of ramp-time on the thermal-fatigue life of SnAgCu lead-free solder joints.” In IEEE Proceedings of Electronic Components and Technology Conference, Lake Buena Vista, FL, May 31–June 3, 2005, pp. 1292–1298. 129. Yu, D., Chai, T., Thew, M., Ong, Y., Rao, V., Wai, L., and Lau, J. H. “Electromigration study of 50 μm pitch micro solder bumps using four-point kelvin structure.” In IEEE Proceedings of Electronic Components and Technology Conference, San Diego, CA, May 2009, pp. 930–935.
CHAPTER
4
Advanced MEMS Wafer-Level Packaging 4.1
Introduction Microelectromechanical systems (MEMS) technology has been investigated widely and vigorously by the research community for various applications over the past few years. Key factors for commercial success in MEMS devices include cost, yield, and reliability. Wafer-level packaging offers advantages and limitations that are substantially different from those of conventional packaging technology. Wafer bonding and wafer-level encapsulation enable a sealed and protected cavity for suspended MEMS structures. Planar and vertical electrical interconnects are selectively prepared by using micromachining technology. The greatest promise of wafer-level packaging appears to lie in the functional areas of various MEMS sensors, radio frequency (RF) MEMS, and optical MEMS. Owing to its unique nature, low-temperaturesolder-based wafer bonding technology continues to evolve toward a mature and reliable solution for enabling wafer-level hermetic packaging for MEMS. Indeed, wafer-level packaging technology is now poised to offer significant improvements and merits over conventional technology in MEMS packaging. The packaging of MEMS devices is one of the most challenging parts of MEMS commercialization. MEMS devices typically consist of cavities and free-standing or even out-of-plane microstructures, whereas integrated circuits (ICs) do not. Given this major difference between MEMS and IC devices, packaging for MEMS devices must allow space for actuator movement, permit the sensing element to interact with the surroundings via a pathway, or provide a suitable ambient inside the package to achieve higher sensitivity or better reliability. Each particular kind of MEMS device requires a more customized and dedicated solution than just a standard solution that aims at
157
158
Chapter Four packaging for all MEMS devices.1,2 In addition to the aforementioned issues, the common requirements for developing a MEMS package include protection of fragile structures, formation of electrical interconnects, manufacturability, and reliability. The main consideration in MEMS packaging is that the free-standing and fragile MEMS structures either have to be protected properly before the chip singulation step (e.g., saw dicing) or must be strong enough to withstand the saw-dicing step. Generally speaking, suitable technologies for MEMS packages typically need to provide sealing or encapsulation of MEMS structures and electrical feed-throughs and pathways for the MEMS device to interact with the ambient so as either to sense the change or to introduce a change. The huge markets for mobile phones and handheld devices for computing and amusement applications generate new high-volume markets for MEMS microphones, inertial sensors, and RF MEMS devices. All these applications require thin and small packaged devices. Wafer-level packages and wafer-level chip-scale packages have been used widely in the IC-packaging industry. Vertical interconnects and stacking chips are deployed as cornerstone technologies for system-ina-package (SiP) solutions for mass production of some commercially available ICs. The concept of SiP solutions actually can help in the development of MEMS packaging.3,4 While most SiP solutions have relied on wafer-level approaches, wafer-level approaches for enabling MEMS packaging also show advantages in many respects. This chapter surveys the progress of wafer-level MEMS packaging. Some potential future research subjects also will be discussed. Basically, wafer-level MEMS packaging involves major technology challenges in terms of methods of wafer bonding and the formation of electrical interconnections, as well as requirements for hermeticity and/or vacuum. Wafer-level approaches are preferred for MEMS packages because approaches at this stage are considered to be batch-type processes, and they typically protect the microstructures from the potential damage during the die-separation step. Besides, the know-good-die testing, die marking, and die separation can be done at the wafer level. Most of packaging and assembly steps for MEMS devices after that can be realized by leveraging the existing techniques in IC packaging. Thus the cost of packaging MEMS device is drastically reduced, whereas the packaging yield is apparently increased.
4.2
Micromachining, Wafer-Bonding Technologies, and Interconnects 4.2.1 Thin-Film Technologies The evolution and maturity of MEMS in recent years have been driven by continuous progress in fabrication facilities and process development.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g Traditionally, there have been two types of micromachining: bulk and surface micromachining. With strong demand for the development of complicated three-dimensional (3D) optical MEMS applications, enormous efforts have gone into integration of multiple and mixed process technologies. Unique integrated process technologies come from combining steps based on bulk and surface micromachining, wafer-bonding technology, and basic semiconductor fabrication techniques. These semiconductor fabrication techniques are (1) thin-film deposition, (2) lithography, and (3) etching. Thin films are deposited using various chemical or physical techniques and are used for masking, insulation, and structural purposes. Subsequent to thin-film deposition, the lithography step is performed such that the designed patterns are transferred from the mask to the substrate. Then substrate with photoresist patterns is etched using various wet-chemical and dry-plasma etching approaches. Finally, patterns of multiple thin layers on the substrate are fabricated after a number of steps including these three major techniques. To facilitate an understanding of the full range of MEMS fabrication technology, we start with the introduction of various micromachining technologies.
4.2.2
Bulk Micromachining Technologies
Bulk micromachining is deployed to selectively remove significant amounts of silicon from a silicon substrate. The geometries of etched features lie along a continuum between fully isotropic and anisotropic. Wet anisotropic etching is currently by far the most commercially successful method used to manufacture devices such as pressure sensors and ink-jet print heads. Wet anisotropic etch agents are ratelimited, whereas wet isotropic etch agents are diffusion-limited. Both involve oxidation of the Si followed by dissolution of the hydrated silicate. The most common wet isotropic silicon etch solution is HNA, which stands for a mixture of hydrofluoric acid (HF), nitric acid (HNO3), and acetic acid (CH3COOH). The HNO3 drives the oxidation of the silicon, and the acetic acid helps to prevent the dissociation of HNO3 into NO3– or NO2–. The etching chemistry is complex (owing to theautocatalytic ionization of HNO3), and etch rates also depend on the chemical mixture and doping concentration of silicon. The fluoride ions from HF react to form the soluble silicon compound H2SiF6. The overall reaction1 is given by 18HF + 4HNO3 + 3Si → 3H2SiF6 + 4NO(g) + 8H2O
(4-1)
Owing to equal etch rates in all directions, the HNA is used to round the sharp corners, to remove the roughness, and to perform the thinning. The main function of the isotropic wet etch in bulk micromachining is to remove the underlying silicon substrate or the silicon sacrificial layer. As a result, the free-standing structures are
159
160
Chapter Four released from the substrate and remain on top of an isotropically etched cavity or a sacrificial gap. A useful formulation for HNA is 250-ml HF, 500-ml HNO3, and 800-ml CH3COOH.2 When HNA is used at room temperature, an etch rate of 4 to 20 μm/min is obtained, and this is increased with agitation. The HNA wet etch can be masked with silicon nitride or silicon dioxide (however, the silicon dioxide film is attacked rather quickly at a rate of 30 to 70 nm/min). It is also noteworthy that the HNA etch rate becomes slower by 150 times in the regions of light doping (<1017 cm–3 n- or p-type) than in more heavily doped regions. Second, the anisotropic etchants etch much faster in one direction than in the other, exposing the slowest-etching crystal planes over time. The slowest-etching crystal planes {111} lead to sloped sidewalls of 54.7 degrees, that is, the angle between the (111) plane and the wafer’s surface of the (100) plane of the {100} silicon wafer. To facilitate concept development in silicon crystal orientation, the four types of commercially available silicon wafers are illustrated in Fig. 4-1a, whereas various planes in a {100} n-type silicon wafer are sketched in Fig. 4.1b. Depending on the dimensions of the mask opening, a V-groove or trapezoidal basin is formed in the [100] wafer, as shown in Fig. 4-1c. A large enough opening will allow the silicon to be etched almost all the way through the wafer, leaving a thin dielectric membrane on the other side. Backside etching can be used to create free-standing structures such as beams, membranes, and plates. The three most important anisotropic silicon etchants are potassium hydroxide (KOH), ethylene diamine pyrochatechol (EDP), and tetramethyl ammonium hydroxide (TMAH). These etchants attack silicon along preferred crystallographic pathways. The crucial difference between these etchants is in the etch rates and hard-mask materials to be deposited on the substrate. Suitable hard-mask materials for KOH are silicon nitride and silicon carbide, which etch at negligible rates. In contrast, silicon dioxide is not an ideal mask materials for KOH owing to an etch rate that is typically 1/200 of the etch rate of {100} silicon plane. The KOH is corrosive to aluminum. Thus refractory metals (e.g., gold) are used as the metal surface to be exposed to KOH solution. However, silicon dioxide can be used as a hard mask when etching with TMAH because the etch rate is negligible. This is a clear advantage of TMAH anisotropic etching for releasing dielectric layers from a substrate made by the standard CMOS process. Another advantage of TMAH anisotropic etching is that it is possible to reduce the etch rate of aluminum to an acceptable level by adding silicon and/or polysilicic acid3 or by adding (NH4)2CO2 or (NH4)HPO4 to the etchant to lower the pH.4 The drawback to this TMAH etching condition is that hillocks and rough surfaces are generated in the {100} silicon planes. These can be alleviated to some extent by the addition of an oxidizer (e.g., ammonium peroxydisulfate).5
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g Secondary flat
No secondary flat (111) p-type
90° 45°
y
Primary flat
t fla
Primary flat
(111) n-type
(100) p-type
ar nd co Se
Secondary flat
(100) n-type
Primary flat
Primary flat
(a) (010) plane
(100) plane
(001) plane
tio n
z, [001] y, [010] x, [100]
(110) plane
[11 0] dir ec
45°
(110)
(b)
(111)
[001] [010] (111) [100]
(111)
Surface is (001)
(111)
Flat is along [110] direction
(c)
FIGURE 4-1
(a) Drawings showing the primary and secondary flats of {100} and {111} wafers for both n- and p-type doping. (b) Various planes in a wafer of {100} orientation (the wafer thickness is exaggerated). (c) Perspective view of a {100} wafer and a KOH-etched pit bounded by {111} planes. (Reprinted with permission from Maluf, N., and Williams, K., An introduction to microelectromechanical systems engineering, 2nd Edition, London: Artech House, 2004, ISBN 1-58053-590-9, Copyright 2004 Artech House.)
In the case of EDP anisotropic etching, both silicon dioxide and silicon nitride can be used as hard masks. In addition, many metals are not attacked by EDP, except aluminum, although the etch rate of aluminum for some formulations of the etchant can be reduced to useful proportions.6 It is also reported that the silicon etch rates versus temperature for the EDP formulation given above are 14 μm/h at 70°C, 20 μm/h at 80°C, 30 μm/h at 90°C, and 36 μm/h at 97°C.6 However, EDP is extremely hazardous, very corrosive, and carcinogenic, and it has to be used in a reflux condenser.
161
162
Chapter Four The silicon etching mechanism involved in these anisotropic etchants is suggested as the following reaction sequence.7,8 First, silicon atoms at the surface react with hydroxyl ions. The silicon is oxidized to form Si(OH)22+, and four electrons are generated as Si + 2OH– → Si(OH)22+ + 4e–
(4-2)
By taking these four electrons, water is reduced to form hydroxyl ions and hydrogen gas; that is, 4H2O + 4e– → 4OH– + 2H2
(4-3)
The Si(OH)22+ further reacts with hydroxyl ions to form a soluble SiO2(OH)22– and water; that is, Si(OH)22+ + 4OH– → SiO2(OH)22+ + 2H2O
(4-4)
The overall reaction is sum up as Si + 2OH– + 2H2O → Si(OH)22+ + 2H2
(4-5)
A thorough overview of alkaline etchants, their properties, and their mechanisms can be found in Seidel and colleagues.8 As a reference, the paper reports that the (100) silicon etch rate is derived as 1.4 μm/min for a 50 wt% KOH solution at 80°C.1 KOH wet etching solution concentrations below 20 wt% are not used because of the high surface roughness and the formation of potential insoluble precipitates. In addition, such solutions all show a marked reduction in etch rate in heavily doped (>5 × 1019 cm3) boron ( p++) regions that are formed by ion implantation and diffusion. This greatly simplifies the tooling required to perform the etch. However, the etch-rate selectivity is not quite as high as for passivating oxides. Besides, the p++ diaphragm shows residual tensile stress that might affect the performance of devices. Chemically reactive vapors and the reactive species in glowdischarge plasmas are highly effective etchants. These are known as dry-etching-process technologies and are classified into two groups: vapor etching and plasma-assisted etching. Plasma-assisted etching has been a key process in the semiconductor and optoelectronics industries for more than three decades. Given the well-established industrial infrastructure in terms of equipment makers and users and available technological knowledge and process recipes, plasmaassisted etching is the dominant process technology in the MEMS industry as well. Plasma-assisted etching has several advantages over the wet etching techniques. It normally offers smaller undercut (allowing smaller lines to be patterned) and higher anisotropicity (allowing high-aspect-ratio vertical structures) than wet etching, but the etchrate selectivity in some cases is not as good as that in wet etching.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g There are three basic dry-etching techniques, namely, high-density plasma etching, reactive-ion etching (RIE), and ion milling (ionbombardment etching) in ref 9. The shape of a plasma-assisted etched feature is a strong function of the etching conditions. The least selective use of ions produced in a plasma is for the sputtering away of material. This is known as ion milling or ion-bombardment etching. When a blanket opening is exposed to plasma (e.g., argon plasma), the energetic argon ion ejects atom from the exposed surface owing to the ion-bombardment effect (or sputtering). Sputtering rate generally is low because the yield typically is like “one atom per incident ion,” and ion fluxes incident on surfaces in discharges are often small. Ion milling is a wellestablished technology and not a mainstream mass-production technology in the industry. Nevertheless, it is an effective approach for removing nonvolatile materials from substrate surfaces. In low-pressure glow-discharge plasmas, energetic ions are accelerated across the plasma sheath edge and strike the surface vertically with kinetic energy, resulting in directional etching (i.e., good anisotropy and poor selectivity). Thus the higher the base pressure in the plasma, the more isotropic is the etch profile owing to a much shorter mean free path of ions. In contrast, the etch rate generally is reduced in a plasma reactor chamber at lower pressure, whereas the etch becomes more directional because the ions that are accelerated through the dark space at the edge of the plasma strike the surface with a definite orientation. By leveraging the reactive chemical species (e.g., gas-phase etchant atoms or molecules such as the F atom in silicon etching) at the surface of the area to be etched, RIE leads to higher etch rate than the sum of the chemical etching rate and the sputter etching rate operated individually. In other words, RIE can remove surface material by direct ion bombardment and chemical-reaction effects, whereas the etched surface atoms are converted to volatile species that can be removed by the vacuum pump connected with the reactor chamber. Because of a lesser ion-bombardment effect in RIE, sidewalls are not etched significantly; that is, the ions do not strike sidewalls mainly. As a result, RIE provides much better directional etching. The tradeoff between anisotropy and selectivity is important in designing etch parameters in an RIE process. Given the significant effort made in silicon semiconductor manufacturing, there is a rich combination of plasma chemistries that can be used for etching all the microelectronic thin films: oxides, nitrides, metals, and silicon. A relevant selection to silicon micromachining is suggested in Table 4-1. To provide a better sense in process design, wet-etch alternatives are listed for a fair comparison. A much more complete database of etchants, including data on etch rates and selectivity, can be found in ref. 1. Most etch chemistries involve either fluorinated or chlorinated species. Recipes are developed to achieve the desired chemical selectivity, for example, etching oxide and stopping on nitride or etching silicon and stopping on oxide, whereas the etched profile is a main concern as well (i.e., the anisotropy).
163
164 Wet Etchants (Aqueous Solutions) Thermal silicon dioxide
LPCVD silicon nitride
Etch Rate (nm/min)
Dry Etching Gases (Plasma or Vapor Phase)
Etch Rate (nm/min)
HF
2,300
CHF3 + O2
50–150
5NH4F:1HF (buffered HF)
100
CHF3 + CF4 + He HF vapor (no plasma)
250–600
SF6
150–250
CHF3 + CF4 + He
200–600
Hot H3PO4
5
66
Warm H3PO4:HNO3:CH3COOH
530
Cl2 + SiCl4
100–150
HF
4
Cl2 + BCl3 + CHCl3
200–600
Gold
KI:I2
660
Titanium
HF:H2O2
110–880
SF6
100–150
Tungsten
Warm H2O2
150
SF6
300–400
K3Fe(CN)6:KOH:KH2PO4
34
Chromium
Ce(NH4)2(NO3)6:CH3COOH
93
Cl2
5
Photoresist
Hot H2SO4:H2O2
>100,000
O2
350
CH3COOH3 (acetone)
>100,000
Aluminum
(Reprinted with permission from Maluf, N., and Williams, K., An introduction to microelectromehcanical systems engineering, 2nd Edition, London: Artech House, 2004, ISBN 1-58053-590-9, Copyright 2004 Artech House)
TABLE 4-1
Wet and Dry Etchants of Thin Metal Films and Dielectric Insulators
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g Other than the dry-etching mechanisms introduced earlier (e.g., ion-bombard etching and RIE using capacitively coupled parallelplate electrodes), the last mechanism, and perhaps the most important dry-etching technique used in bulk micromachining, is high-density plasma etching. By using inductively coupled plasma (ICP) or an electroncyclotron resonance (ECR)–based power source, the high-density plasma reactor can independently control plasma parameters such as electron energy, ion energy, and plasma density. The high-density plasma reactor operates at lower process pressures and achieves a high ionization ratio such that the density of the plasma is higher than that of capacitively coupled plasma because the high-density plasma reactor can efficiently transfer energy to electrons so as to achieve a high ionization ratio. Furthermore, the longer mean free path of ions in the lowpressure process in a high-density plasma reactor enables significant improvements in directional etching. Therefore, high-density plasma etching is called deep reactive ion etching (DRIE). Starting in early 1990s, research attempts were focused on advanced DRIE in order to develop bulk micromachined structures with very high aspect ratios. One approach was for the glow discharge to supply the etchants, energetic ions, and inhibitor precursor molecules. Most plasma processes are a critical race between deposition of polymeric material from the plasma and removal of material from the surface. In well-designed plasma chemistries, removal (i.e., the etch process) dominates. By using a cryogenic cooling technique, when a wafer is maintained at liquid-nitrogen temperatures, the reactant gases condense onto the silicon surface, thus passivating the surface. For example, the inhibitor precursor molecules (e.g. CF2, CF3, CCl2, and CCl3), which are called unsaturates, deposit on the substrate surface to form fluoro- or chlorocarbon polymer films (i.e., a protective layer). In such DRIE equipment, the ion-bombardment effect is suppressed, but just enough for removal of the polymer layer on the bottom surfaces of etched trenches so as to perform the reactive ion etching continuously, whereas the polymer layer on the sidewalls of the trenches is retained owing to the directional ion etching effect (i.e., energetic ions move along the direction normal to the substrate). SF6 typically is used because of the high etch rates that can be achieved. The passivation can be enhanced by the addition of oxygen to the plasma, which results in an increased ratio of fluoro- to carbon, meaning more fluorounsaturates for polymer passivation. A potential problem with the cryogenic approach involves maintaining the cryogenic temperature of all the microstructures during the etch process. Some microstructures may become thermally isolated from the substrate when they are released from the substrate and become free-standing. The raised temperature in the local freestanding microstructures may lead to deterioration of polymer passivation. When polymer passivation on these microstructures is not sufficient, the etching mode dominates. As a result, notching and RIE
165
166
Chapter Four
C4F8
Photoresist
Scallop SF6
CF2 species for passivation
F species for etching
(a)
(b)
Photoresist
Silicon 10 μm (c)
1 μm (d)
FIGURE 4-2 Profile of a DRIE trench using the Bosch process: (a) passivation step of using CF2 species; (b) fluoroion-based etching step; (c) SEM microphotograph of cross-sectional view of DRIE trenches; (d ) SEM microphotograph of close-up view of scalloped sidewall. The process cycles between an etch step using SF6 gas and a polymer deposition step using C4F8. The polymer protects the sidewalls from etching by the reactive fluorine radicals.
lag effects are observed in this case such that the uniformity of etching results is not good. Scientists at Bosch have developed a revised process to further improve process control in DRIE.10 Instead of relying on the balance between plasma etching and polymer passivation, the Bosch process uses alternate etching and passivation steps, as shown in Fig. 4-2. The passivation is achieved by deposition of a polymer using CFx+, which is decomposed from C4F8 feedgas. The subsequent step is a reactiveion etching process using such species as F+ and SFx+, whereas the polymer on the bottom of the trench is removed owing to the directional etching effect of ion bombardment. The normal cycle time for each deposition or etch step is a few seconds. The resulting etch rate is 1 to 15 μm/min typically. An aspect ratio of etched trench of 30:1 can be achieved. A comparison of DRIE technology with other bulk micromachining technology is given in Table 4-2. The general issues
HF:HNO3: CH3COOH
KOH
EDP
N(CH3)4OH (TMAH)
SF6
SF6/C4F3 (DRIE)
XeF2
Etch type
Wet
Wet
Wet
Wet
Plasma
Plasma
Vapor
Typical formulation
250-ml HF, 500-ml HNO3, 800-ml CH3COOH
40 to 50 wt%
750-ml ethylenediamine, 120-g pyrochatechol, 100-ml water
20 to 25 wt%
Anisotropic
No
Yes
Yes
Yes
Varies
Yes
No
Temperature
25°C
70–90°C
115°C
90°C
0–100°C
20–80°C
20°C
Etch rate (μm/min)
1–20
0.5–3
0.75
0.5–1.5
0.1–0.5
1–15
0.1–10
[111]/[100] Selectivity
None
100:1
35:1
50:1
None
None
None
Nitride etch (nm/min)
Low
1
0.1
0.1
200
200
12
SiO2 etch (nm/min)
10–30
10
0.2
0.1
10
10
0
p + + etch stop
No
Yes
Yes
Yes
No
No
No
Roomtemp. vapor pressure
167
(Reprinted with permission from Maluf, N., and Williams, K., An Introduction to Microelectromehcanical Systems Engineering, 2nd Edition, London: Artech House, 2004, ISBN 1-58053-590-9, Copyright 2004 Artech House).
TABLE 4-2
Liquid, Plasma, and Gas Phase Etchants of Silicon
168
Chapter Four in both DRIE processes is that the etch rate is a function of the density of the opening area and trench width. Investigation of an etched dummy wafer is necessary for etch-rate calibration when users have a new lithography mask layout. Another dry bulk micromachining approach is vapor-phase etching. A reactive gas mixture that typically contains fluorine can etch silicon with very high selectivity to many masking layers, including Al, SiO2, Si3N4, photoresist (PR), and phosphosilicate glass (PSG). One of the most widely employed reactive gases is XeF2. As suggested by Chang and colleagues,11 the reaction with silicon is given by 2XeF2 + Si → 2Xe + SiF4
(4-6)
The gas xenon diflouride performs the non-plasma-based isotropic etch of the solid silicon surface and forms the volatile SiF4 product. This etch reaction completes with desorption of the volatile SiF4 product and residual xenon from the silicon surface. It is noteworthy that the etched surfaces shows granular structures of a few microns, making the etched surface unsuitable for situations where smooth surfaces are required (e.g., optical reflection surfaces). This reaction is exothermic. Thus the generated heat may adversely influence some microstructures. Pulse-mode operation of XeF2 etching is suggested. An important concern is that XeF2 reacts with water (even moisture in air) to form Xe and HF, whereas the generated HF will unintentionally etch silicon dioxide. A properly designed reaction chamber linked with a vacuum pump is still required for handling XeF2 vaporphase etching. The typical etch rate is a few micrometers per minute, as shown in Table 4-2. It is ideal for the dry release of CMOS MEMS devices (i.e., dielectric layers from a CMOS substrate) and surface micromachined structures in which polysilicon is used as the sacrificial layer.
4.2.3
Conventional Wafer-Bonding Technologies for Packaging
Wafer bonding is used widely in MEMS fabrication and packaging.12 It refers to approaches of firmly joining two wafers (or more) to create a stacked and bonded wafer. There are three main kinds of waferbonding processes: direct bonding, field-assisted bonding, and bonding with an intermediate layer. The choice of which is most suitable depends on the particular application and the materials involved. Silicon-to-silicon direct bonding, also called fusion bonding, is a direct silicon-to-silicon bonding technique without the assistance of significant pressure or any intermediate layers or fields.13 The process requires rather flat and clean surfaces as the bonding interface for the two wafers. The surfaces of silicon wafers are cleaned and rinsed first. Hydroxyl (–OH) groups form on the surfaces of the two wafers with
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g a thin native silicon oxide layer (i.e., hydrophilic surface). Two wafers can be joined together at room temperature, resulting in an immediate weak bond owing to van der Waals forces. Then the bonded wafers are heated to 800 to 1000°C to remove the water molecules and leave behind Si–O–Si bonds at the interface. Owing to perfectly matched thermal-expansion coefficients of the two wafers, silicon direct-bonded wafers have little or no residual stress owing to thermal mismatch. However, silicon direct bonding normally is used as the beginning step in an integrated process because of the rather high annealing temperature and high-quality requirement of the bonding interface in terms of cleanness and flatness. Another direct-bonding technology is restricted to bonding glass to a conductive substrate using electrical bias, that is, field-assisted bonding or anodic bonding.14 A glass wafer with a high concentration of sodium ions (e.g., Pyrex 7740 glass from Corning) is biased as the cathode, and the silicon wafer is the anode. The contacted wafers are heated to 300 to 400°C, and a voltage of about 200 to 1000 V is applied. The applied voltage produces a very high electrostatic attractive force that pulls the silicon and glass into intimate contact. The sodium ions in the glass wafer (i.e., the cathode side) diffuse toward the opposite side from the bonding interface, whereas the oxygen ions of negative charge are left behind and accumulate at the bonding interface. The available oxygen ions and silicon atoms at the interface will form strong Si–O bond, whereas a current of a few milliamperes per square centimeter flows between the two electrodes, signifying the movement of ions and completion of the process. When bonding is completed, this current drops to zero. Similar to the concern we have in silicon direct bonding, the anodic bonding is very susceptible to interference from particulate contaminants. To achieve an anodic bonded interface of good quality, there are several parameters, such as surface preparation, contact load, temperature, time of applied voltage, and magnitude of the applied voltage, that should be monitored during the bonding process. A number of glasses from different vendors can be used in anodic bonding. Basically, conductive glasses with a reasonably high content of sodium and boron have lower melting and softening temperatures. These glasses are more suitable for anodic bonding. When the glass is purer, its electrical conductivity decreases, which reduces the electric field strength and lowers the electrostatic attraction that exists between the two wafers. As a result, glass substrates of lower conductivity typically need a higher bonding temperature and a higher biased voltage to achieve a successful bond. A wide range of intermediate layers has been used for wafer-towafer bonding in microstructure fabrication. These intermediate-layer bonding approaches include eutectic bonding, glass-frit bonding, solder-based thermocompression bonding, and adhesive bonding. Eutectic bonding deploys a thin gold layer as an adhesive layer to
169
170
Chapter Four bond silicon wafers.15 The wafers, coated with a thin gold layer, are brought into contact at a temperature higher than Au-Si eutectic point (i.e., 363°C for 2.65% Si in Au). The common practice is bonding at 370°C for 15 minutes under 7 kN of applied force using a commercially available bonding tool. Wafer-level packaging based on a glassfrit-sealed interface between the MEMS wafer and a cap wafer has been a major technology for volume production of MEMS accelerometers in automotive airbag systems to realize hermetic sealing. This method is similar to the long-established approach of glass frits as seals in conventional hermetic ceramic packages.16 The cap wafer is stenciled with a mixture of glass and binder and patterned to form the walls of each device cavity. Another cap wafer is aligned and thermocompression bonded to the device wafer with glass-frit bonding rings. The bonding condition typically requires a temperature higher than 400°C and an applied pressure of 2 bars. However, reliable sealing using glass frits requires a relatively wider wall-sealing pattern. This implies fewer gross dies per bonded wafer. Eutectic Au-Sn solder has long been recognized as an approach offering superior high-temperature performance, high mechanical strength, and fluxless soldering because the melting temperature of its eutectic composition (Au 30 at% Sn) is 280°C.17,18 This approach has been used widely in the optoelectronics and microelectronics industries. It is a reliable solution for packages comprised of sealing of a Kovar case to a ceramic substrate. However, there is concern that a large residual stress will be introduced when two bonded wafers with a relatively large difference in coefficient of thermal expansion (CTE) undergo a process with a large temperature difference. In addition to the above-mentioned wafer-bonding technologies using the intermediate layer for hermetic bonding, the last group is polymer-based adhesive bonding. First, polymer-based adhesive bonding is used as temporary bonding of wafers, where the polymer just has to keep the wafers together during the micromachining process. Second, polymer-based adhesive bonding can be used to form waferbonded structures in nonhermetic and near-hermetic packages. Various kinds of adhesives, including epoxies, poly(methylmethacrylate) (PMMA), polyimides, silicone rubbers, and negative photoresists, are used. Generally, such polymer bonds can be achieved at temperatures lower than 150°C. Thus there is no serious concern about residual stress owing to the thermal-expansion mismatch between different types of wafers in the bonded wafers.19 Two polymer materials with major research interests are SU-8 and benzocyclobutene (BCB). SU-8 is an epoxy-based negative-resist material from Microchem, whereas BCB is from the Dow Chemical. BCB shows minimal outgassing, low moisture uptake, and excellent electrical properties. In one process, as shown in Fig. 4-3, BCB is spincoated onto the capping wafer and photopatterned to provide sealing
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g
Si Si
(a)
BCB intermediate bounding layer
(b) (e)
Spacing created by using dicing saw
(c) Si cap
(d)
PCB
(f)
FIGURE 4-3 Wafer-level packaging approach using polymer as the intermediate layer to form the sealing interface, ref. 21.
rings. After the cap wafer is bonded with the device wafer, multistep dicing is used to expose the bonding-pad area and separate each die from the bonded wafer (see Fig. 4-3b and c). For example, the capped die can be die-bonded and wire-bonded on a PCB. Thereafter, the whole packaging process is accomplished by a molding step (see Fig. 4-3d). The bonded wafer after dicing and a close-up view are shown in Fig. 4-3e and f, respectively. The reflow characteristic of BCB during the curing step allows the planar electrical signal feed-throughs passing through the bonding ring while maintaining a good seal. RF MEMS switches and film bulk acoustic resonator (FBAR) filters have been packaged by using the BCB capping process.20,21 On the other hand, we do not want residual BCB left inside deep cavities for wafers with high-aspect-ratio cavities; thus, we should not use a spin-on step to prepare the BCB coating layer. Besides, we could not use the spin-on process to prepare the BCB coating layer on a wafer with free-standing structures. A new process called contact printing provides better results than the spin-on technique. The contact printing method uses viscous BCB as “ink” and a soft-cured BCB pattern as a stamp to improve the bond strength of full-wafer adhesive bonding with patterned BCB as the intermediate bonding layer. This technology successfully demonstrated that the bond strength of samples has been improved by a factor of 2 over the conventional spin-on BCB bonding technique.22,23
171
172
Chapter Four
4.2.4
Plasma-Assisted Wafer-Bonding Technologies
Another low-temperature direct bonding approach is known as plasma-activated wafer bonding or surface-activation bonding. The plasmaactivation step modifies the surface chemistry in a similar manner to hydrophilic surface treatment. The substrates are pretreated with plasma and cleaned off, and then they are brought into contact with or without external pressure and high temperature to form an irreversible bond.24,25 Plasma may be generated from different feedgases, including oxygen, argon, nitrogen, and hydrogen. Oxygen plasma creates a thin oxide layer on the interface and is used for applications that require electrical isolation at the interface. On the other hand, hydrogen, nitrogen, and argon plasmas are used in applications where a bonded interface is preferred that does not have a residual oxide layer. Obviously, this process has to be carried out in a vacuum environment (i.e., a plasma chamber such as an RIE chamber or an ICP chamber). It is also possible to treat the surfaces chemically using a barrier-discharge method, where plasma is formed in the atmosphere. Plasma-activated bonding now has been applied to various materials, including silicon, compound semiconductors, oxides, and polymers.25 Normally, an annealing step at an elevated temperature of 100 to 400°C is needed depending on the required bond strength and the materials being bonded. When the wafer surface is cleaned using argon-beam sputtering in a high-vacuum environment, silicon wafers can be bonded at room temperature.26,27 The type of plasma used to activate the bonding surface, plasma power, and the annealing step all can have a significant influence on bond strength and void or defect density at the interface. Because wafers need to be aligned and then bonded in the plasma chamber without breaking vacuum, specialized alignment and bonding stages, as well as the substrate heater, need to be included in a single machine.
4.2.5
Electrical Interconnects
The most common electrical interconnects are the planar electrical leads. They are typically prepared on the same side of MEMS wafer. There are two major kinds of planar electrical leads: buried leads and surface leads. Buried leads can be heavily doped Si or metal silicide (e.g., AlSi) that forms a low-resistive path on the silicon substrate. For the surface lead line, the Al-alloy process used in microelelctronics is a common solution for MEMS (see Fig. 4-3). However, the Al may need to be substituted by other materials that can withstand the hightemperature process. Highly doped polysilicon is used commonly as a lead-line material in the surface micromachining technology, and it can sustain in all kinds of high-temperature wafer-bonding processes using the intermediate layer. Generally speaking, highly doped silicon or polysilicon is used widely as lead lines in electrostatic actuated
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g MEMS and capacitive sensors. It should be noted, though, that polysilicon leads typically exhibit higher 1/f noise than metal leads. Thus, in some resistive types of MEMS sensors, polysilicon leads may not be a good choice. Second, anisotropic wet-etched Si V-grooves could be used for through-wafer vertical electrical vias when metal leads are sputtered or electroplated on the V-groove sidewalls. Owing to the angle of the V-grooves, the footprint of through-wafer V-groove vias is relatively larger, as shown in Fig. 4-4a.28 Since the size of the through-wafer V-groove vias is determined simply by the thickness of wafer, by using a thin device layer of a silicon-on-insulator (SOI) wafer, the V-groove vias can be shrunk to a very small area (see Fig. 4-4b and c).18
(a) Electrical interconnects
μ-via
Solder ball (b)
V-groove μ-via SMD pad
Sealing ring
μ-via
(c)
FIGURE 4-4 V-groove type of vertical interconnects with small footprint for wafer-level MEMS packaging.
173
174
Chapter Four On the other hand, through-wafer vertical holes of silicon and glass substrates can be created by using DRIE or photo-assisted electrochemical etching. After forming the insulation layer based on thermal oxidation, chemical vapor deposition (CVD) dielectric-layer coating, or CVD parylene coating, the through-wafer vertical interconnects can be formed by heavily doped polysilicon conformal deposition, metal sputtering, metal plating, or vacuum metal sucking and refilling.29–32 Combining the vertical interconnects with cavities on the cap wafer allows the formation of a large number of interconnects and wafer-level packaging by means of a simple bonding step at the same time. In particular, wafer-level packaging using a solder intermediate layer with reflow is very suitable to this approach because the solderreflow step will enhance the connection between the vertical interconnects of the cap wafer and the planar electrical pads of MEMS wafer both mechanically and electrically. As shown in Fig. 4-5, this concept has been applied to the vacuum sealing of accelerometers (see Fig. 4-5a and b) and the hermetic sealing of RF MEMS switches (see Fig. 4-5c and d).33,34 Without using the high-temperature thermal oxidation process, a novel low-temperature process of creating a thick SU-8 dielectric isolation between Cu vertical interconnects and surrounding Si sidewalls has been reported.35 This approach allows one to create vertical interconnects on a wafer after MEMS devices
Transmission line Piezoelectric actuator
Via hole
Cap wafer
Vacuum Cap substrate
MEMS device Contact electrode
(a) Bottom substrate
Accelerometer device
(c) Via hole Electrode
Copper via
CPW line Bonding material Cap substrate
Cap wafer
Sealing rim
Solder ball Bottom substrate
Substrate (PCB)
(b)
Piezoelectric film
(d)
Contact electrode
Dielectric membrane
FIGURE 4-5 Through-wafer vertical interconnects with solder joints formed at the same wafer-bonding step for solder-based wafer-bonding MEMS packaging.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g or Al planar electrical leads have been prepared on the same wafer. Additionally, the vertical interconnects are quite useful for SiP applications with high input-output (I/O) pin counts.
4.2.6
Solder-Based Intermediate-Layer Bonding
The choice of the intermediate bonding layer is made based on the types of substrates to be bonded, the thermal budget of the process temperature, and whether hermetic sealing is required or not. The well-known intermediate-layer bonding techniques include the use of polymer-based bonding at temperatures ranging from 100 to 150°C, Au/Sn solder–based eutectic bonding at 280°C,17,36 Au/Si eutectic bonding at 365°C,37 and glass-frit bonding at 400°C. Given that most of applications require hermetically sealed packages, polymer-based intermediate-layer bonding produces a gas-permeable interface and therefore does not meet the hermetic sealing requirements. Thus Au/Sn solder bonding and glass-frit bonding are the mainstream approaches in the MEMS industry nowadays. However, many MEMS devices contain different materials or need to bond substrates containing the electronic part of the device (e.g. CMOS wafers). Thus the difference in thermal-expansion coefficients of the dissimilar materials results in mechanical stress that is in proportion to the process temperature. Therefore, low-temperature wafer bonding is the key to avoiding such residual mechanical stress. To fulfill the requirements for hermetic sealing and low process temperatures, indium and indium-based alloy solders have been reported to be very attractive intermediate-layer materials. The batch-type techniques for preparing the solder pattern on wafers for bonding include stenciling, dip coating, electroplating, and evaporation/sputtering. The technical challenges of this process involve uniformity control of the solder pattern, thickness, and composition. Since the In-Sn material system has a eutectic point at 118°C and pure indium melts at 156.6°C, In-Sn (50/50) solder has been investigated as the bonding intermediate layer for packaging of thermal sensors and infrared imaging sensors.38 A helium-leakage rate less than 1 × 10–8 (torr · liter)/s and tensile strength of 200 kg/cm2 for the bonding interface can be obtained with a bonding temperature of 150°C.39 Au-In-Ni intermediatelayer material has been used for packaging thermal sensor arrays as well.40 The authors of this study suggested a thermocompression approach based on the cold-welding characteristics of indium. In a bonding chamber with a forming-gas environment (e.g., N2 90 percent and H2 10 percent), a shear strength of 72 MPa at the bonding interface can be obtained with a bonding temperature of 195°C for 10 minutes with an applied pressure of 8 MPa. This package shows postbonding temperature stability up to 473°C. On the other hand, In compression bonding has been reported for wafer bonding of vacuum-packaged microbolometers for infrared imaging applications.41–43 Extensive
175
176
Chapter Four studies on low-temperature bonding and the characteristics of the bonding interface on the chip-to-chip scale have been reported44–48 using various bonding-interface materials (e.g., In-Sn, In-Ag, In-Cu, and In-Au). Moreover, the industry also requires solder-bonded interfaces to be able to survive at temperature at least as high as 285°C, which is the peak temperature in the surface-mounting-technology (SMT) manufacturing line. This means that the resulting intermetallic compounds (IMCs) of the solder-bonded interfaces in any postbonding steps need to have a melting temperature (i.e., a remelting temperature) that is higher than the postbonding process temperature. Incorporating In and Sn as the solder layer to react at a high melting temperature to form stable IMCs is a new research direction in low-temperature solder-based wafer bonding that aims to create a materials evolution of the resulting IMCs at the bonded interfaces with respect to various postbonding heat-treatment process conditions. We will discuss this recent progress in Sec. 4.6.
4.3 Wafer-Level Encapsulation Wafer-level encapsulation is an approach that consists of using a sacrificial material to cover the MEMS device and a deposited thin film under tensile stress to encapsulate the MEMS device, followed by removal of the sacrificial layer by wet etching or vapor-phase etching through the opening and then encapsulation of the opening by deposition of a thin film. In the case of encapsulating the opening in a thinfilm reaction chamber under vacuum, the sealed cavity of the MEMS device can be preserved at low vacuum. This concept has been applied to achieve wafer-level packaging for capacitive- and piezoresistivesensing pressure sensors49–51 (Fig. 4-6a and b) based on low-pressure chemical vapor deposition (LPCVD) SiN film sealing and for resonators based on polysilicon-film sealing (Fig. 4-6c).52-53 This process is suitable for sealing surface-micromachined MEMS devices owing to its perfect process integration. To enhance the durability and mechanical robustness of the encapsulation, a 20-μm-thick epitaxial Si layer is prepared using dichlorosilane at 1080°C to seal the MEMS structure first, denoted as the cap layer in Fig. 4-6d. Then trenches are etched through the cap layer to allow the HF vapor etching to remove the refilled SiO2 and release the MEMS structure, thereby isolating the electrical conductive paths.54,55 Finally, a layer of LPCVD oxide is deposited on top of the cap layer to create a seal over the trenches. Since the oxide deposition furnace is under vacuum, the parts are also under vacuum when sealed. After the sealing oxide is deposited, metal layer is deposited and patterned to form the electrical leads and pads. Since SiO2 is permeable to the ambient gases, the silicon nitride film or metal layer on top of the oxide seal location can extend the vacuum life of package.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g SiN diaphragm PolySi piezoresistors
Optional CMOS
Electrode contact
Epi layer
Sealed vacuum cavity
(a)
Poly layer
SOI layer
(e)
Handle wafer
Deflection electrode
Vibrating resonator
(b) Si epilayer
Shell of sealed vacuum cavity
SOI layer
(c)
Seal oxide Aluminum pads
Al contacts Sealing of vents Seal oxide Cap layer Refill oxide Device layer Sacrificial oxide
(d)
Handle wafer
(f)
PolySi
(g)
FIGURE 4-6 Wafer-level packaging approaches using high-temperature processes to form the wafer-level encapsulation.
4.3.1
High-Temperature Encapsulation Process
The last process described in previous section has been further developed by the Bosch Group and Stanford University and was commercialized recently by SiTime (www.sitime.com) for packaging of MEMS oscillators.56 As shown in Fig. 4-6e and f, this technology encapsulates silicon resonators in epitaxially sealed chambers buried under the wafer surface. Recently, an ultracompact encapsulated accelerometer with a die size of 387 × 387 × 230 μm has been demonstrated using this epitaxial Si encapsulation technology, as shown in Fig. 4-6g.57 The first step in the fabrication process is patterning the resonator structure from an SOI wafer with a 10- to 20-μm-thick device layer. An oxide layer is deposited and patterned to cover the resonator structure while providing via openings for electrical contacts. Then a thin epitaxial silicon layer is grown and patterned to get via openings through the oxide layer down to the silicon electrode part of the
177
178
Chapter Four device layer. Using the HF vapor-based etching, a portion of the oxide layer is removed to release the movable parts of the resonator structure. Thus the portion of this oxide layer that is the sacrificial layer, whereas the remaining portion is the insulating oxide layer (see Fig. 4-6e and f ). In the last step, a thick epitaxial silicon layer is grown on top to seal the trenches such that the cavity containing the movable parts of the resonator is sealed with the same degree of vacuum as the process-chamber pressure used in the epitaxial silicon deposition process. The epitaxial silicon grown on top of the oxide layer forms a polycrystalline silicon layer, whereas a single-crystal silicon layer is formed in the area where the oxide has been removed. After surface planarization and formation of contact isolation trenches, the wafer with encapsulated MEMS structures can be used as a starting wafer for further CMOS processing to create monolithically integrated circuits. The MEMS-first front-end wafer-level packaging process completely defines, releases, and seals the resonant microstructures in the front-end processing steps. Thus it provides reliable wafer-level vacuum packaging at low cost. One advantage of using a high-temperature sealing process (i.e., epitaxial Si deposition) to enable the Si oscillators to be embedded inside a sealed vacuum cavity is that the absorbed molecules inside the cavity will be removed during the high-temperature sealing step, just as in the hot baking treatment. Thus the newly released product exhibits excellent performance in terms of ultralow long-term drift of device features and good frequency stability against temperature variation.56
4.3.2
Low-Temperature Encapsulation Process
This high-temperature epitaxial Si sealing process limits material selection for MEMS devices. Some metals and low-temperature oxides cannot sustain their material characteristics under such high temperatures. As shown in Fig. 4-7, a three-mask low-temperature electroplating process has been proposed.58 An electroplated 40-μmthick nickel film is prepared on a sacrificial photoresist layer of several microns first (see Fig. 4-7a, 5). After the photoresist has been removed via access holes (see Fig. 4-7a, 8), the access holes can be sealed by sputtering a metal layer or melting Pb/Sn solder (see Fig. 4-7a, 9 and 10). If the final sealing step is handled inside a vacuum chamber, a sealed vacuum of about 1.5 torr can be obtained. Figure 4-7b and c show a schematic drawing of a sealed Pirani vacuum sensor and electroplated nickel thick-film cap, respectively. One drawback of this process is that the photoresist-removal step may take several hours. Recently, a novel encapsulation technique used a thermal decomposition step within the temperature range of 180 to 260°C to vaporize the sacrificial polymer via a permeable polymer overcoat, resulting in an encapsulated cap made of the suspended polymer overcoat,59 as shown
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g NI
Cr/Al Si 1. Pattern Cr/AI feed-throughs
PR
PR
Si
Si
PR Si
2. Pattern 3. Evaporate Cr/Au 4. Define plating sacrificial PR seed layer mold
NI
NI
PR
PR
Si 6. Strip PR and AU
PR Si 5. Plate Ni
NI
NI
NI
Si
Si
Si
Si
7. Strip Cr/Al
8. Strip PR
9. Sputter Cr/Au
10. Plate Au
(a) Dielectric membrane Package lid
Cr/Pt resistor
Rounded tethers Cr/Au contacts
Polysilicon Polysilicon anchor feed-throughs
(b)
AccW Spot magn WD Exp 500 μm 10.0 kV 3.0 70x 9.3 1 EMAL XL-50 FEG SEM
(c)
FIGURE 4-7 Wafer-level packaging approaches using low-temperature processes to form the wafer-level encapsulation, in ref. 58.
in Fig. 4-8b to d and f. The hermetic sealing can be realized by additional sputtered metal on top of the polymer overcoat (see Fig. 4-8e and g). Moreover, a sealed vacuum of around 1 torr or less can be achieved by conducting the metal hermetic sealing step inside a vacuum chamber. There are several advantages to this technology, such as 1. Low-temperature processing. The technology is suitable for packaging of MEMS devices that are sensitive to high temperatures and thermally induced residual stress. 2. Low cost and simple packaging. Both the sacrificial and the overcoat polymers can be made photosensitive. The process does not require cap-to-wafer alignment or a wafer-bonding step. 3. High-yield process. Thermal decomposition of the sacrificial polymer is used instead of etching, which is stictionless, structurally benign, and easily controlled. In summary, recent progress in wafer-level encapsulation technology has proven to be versatile and can be extended to any device that does not need direct physical contact with the ambient
179
180
Chapter Four Embedded cavity Insulator
Si beam
(a) Unity
(b) Polymer overcoat (f) (c)
Gold coating Polymer overcoat Vacuum channel
(d) Metal t Ch
tC
1-μm gap (e)
(g)
Beam 50 μm
FIGURE 4-8 Wafer-level packaging approaches using low-temperature encapsulation steps involving polymer and metal coatings, ref. 59.
(e.g., accelerometers, gyroscope sensors, MEMS resonators, RF switches, varactors, and filters). The footprint of MEMS package using this technology is always smaller than that with the bondedcap approach because it does not require extra bonding area in the bonding ring region. Both planar and vertical interconnects can be realized with this technology.
4.4 Wafer-Level Chip Capping and MCM Technologies In addition to wafer-to-wafer bonding–based packaging solutions, a silicon chip with a V-groove cavity can be used as a cap chip to form a sealing cap on top of a MEMS structure on a wafer. This step can be implemented using the common flip-chip bonding technology. Discrete components such as IC chips and capacitors can be assembled on the wafer by the same flip-chip bonding approach. After chip separation, the diced MEMS chip is a carrier chip that hosts the other function chips that require different process technologies to fabricate. An epoxy-based molding step is used to finish the package for such devices. Module-like devices for such applications as RF MEMS, optical MEMS, and wireless sensor nodes can be created with this approach. This approach reflects the concept of a
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g system-in-a-packaging (SiP) solution. A similar approach uses ceramic substrates with cavities to host MEMS chips and other function chips inside the cavities. The standard high-density interconnect (HDI) process consists of embedding bare die into cavities milled into a base substrate and then fabricating a thin-film interconnect structure on top of the components. Each layer in the HDI overlay is constructed by bonding a sheet of dielectric film onto the substrate and forming via holes through a laser ablation process. The Ti/Cu/Ti metallization used for the die interconnects then is created through sputtering and photolithography.60 A device packaged in this manner is called a multiple-chip module (MCM), and it incorporates epoxy-mounted MEMS chips, ICs, surface-mount capacitors, and thick-film resistors. Combining MCM and HDI technology for optical MEMS packaging has been demonstrated.60 Moreover, electrical interconnects can be realized by wire bonds in an MCMpackaged MEMS pressure sensor.61 Another unique technology deploys localized heating to avoid the potential constraints owing to wafer-bonding temperatures because the wafer-bonding temperature must be compatible with all on-chip components, such as microstructures, metallization lines, and integrated circuitry, when the entire wafer is subjected to the same waferbonding temperature in a wafer-to-wafer bonding process. However, for reliable bonding and a hermetically sealed bonding interface, appropriate wafer-bonding technologies such as Au/Sn solder–based eutectic bonding at 280°C, Au/Si eutectic bonding at 365°C, and glassfrit bonding at 400°C normally are used. With this background as motivation, a microresistive heater is integrated into the bonding area either on the substrate or on the capping wafer. After the wafers are brought into contact, the bond is created by locally heating the bonding area via biasing the integrated microheater.62 Based on the reported simulation data,62 a thermal insulating layer (e.g., an SiO2 film) deposited on the thermally conductive substrate (e.g., silicon) can effectively prevent the temperature-sensitive MEMS components from being affected by the high bonding temperatures generated by the microheater during the heating step. With selection of the appropriate material combinations, Au-Si eutectic bonding, Si-glass fusion bonding, and indium solder bonding have been used for demonstrating this localized heating and bonding concept. Either in the wafer-based batch-type process or the chip-based approach, the techniques for preparing the solder pattern on wafers for bonding include stenciling, dip coating, electroplating, and evaporation/sputtering. The technical challenges of this process include uniformity control of the solder pattern, thickness, and composition. B. H. Stark and K. Najafi reported a molding and transferring technology that provides a way to solve these challenges. They reflowed the solder paste in cavities with accurate volume inside a vacuum chamber so as to convert the solder paste to a discrete solder
181
182
Chapter Four ball in each cavity. Then this solder mold was aligned and bonded with the MEMS device wafer in a vacuum. By bonding at 260°C for 2 hours with Bi/Sn solder, a vacuum-packaged cavity that can withstand 1.5 torr can be achieved.63
4. 5 Wafer-Level MEMS Packaging Based on Low-Temperature Solders: Case Study As discussed in Sec. 4.2.6, formation of the bonding interface at low temperature with low-temperature solder (e.g., indium) has attracted a lot of research attention in the creation of hermetically sealed packaging. In order to withstand higher postbonding process temperatures, high-melting-temperature IMCs formed after low-temperaturesolder bonding are preferred. Stable and high-temperature resist bonding interfaces rely on the formation of IMCs of high melting temperature from a low-melting-point (LMP) component such as In or Sn and a high-melting-point (HMP) component such as Au, Ag, or Cu. Looking into the mechanisms of bonding-interface formation using low-temperature solder, two mechanisms are reported. Pure indium is melted at 156.6°C, as seen in the phase diagram in Fig. 4-9a. Reaction between the melted indium (LMP component) and Au, Ag, or Cu (HMP component) is the first mechanism.44–47
0
10
20
Atomic percent indium 30 40 50 60 70
80
90
100
1000 961.93°C 900
Temperature, °C
800 700
670°C
695°C β
L
680°C
600 500 ζ
(Ag)
400 300
187°C
100
α′
205°C 166°C AgIn2
200
γ
0 0 Ag (a)
10
20
30
40
50
60
166.634°C 144°C
70
80
(In)
90
Weight percent indium
FIGURE 4-9 (a) The In-Ag phase diagram. (b) The In-Sn phase diagram.
100 In
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g Weight percent tin 0
10
20
30
40
50
60
70
80
90
100
250 95.7 224°C 200
231.9681°C
L
Temperature, °C
156.634°C 14 10 12
150
120°C 44 48.3
100 β
(In)
γ
50 (βSn)
(αSn)
0 0 In
10
20
(b)
30
40
50
60
70
80
90
130°C
100 Sn
Atomic percent tin
FIGURE 4-9 (Continued )
In-Sn eutectic solder bonding without reaction to form the highmelting-point IMCs is the second approach38,39 (Fig. 4-9b). Considering the bonding temperatures and the formation of void-free joints and reliable IMCs, Sn/Au and In/Au systems have been studied extensively.64,65 Section 4.5.1 will report our recent results of investigations into the reliable high-melting-point IMCs in the In/Ag system for wafer-bonding-based MEMS packaging applications. More important, the use of Au would lead to a high cost for wafer bonding. Compared with Single-component solder of Sn or In, the In-Sn alloy is very attractive because of its low eutectic temperature (118°C) and good wettability with various common substrates. Since Cu is used widely in modern IC packaging technology and in 12-in CMOS process technology and is much cheaper than Au, Sec. 4.5.2 will report on the use of In-Sn of eutectic composition for Cu-based metallization.
4.5.1
Case Study: In/Ag System of Noneutectic Composition
In the In-Ag phase diagram (see Fig. 4-9a),66 the eutectic temperature is seen to be 144°C at 96.5 wt% In, whereas the melting temperatures of indium and silver are 156.7 and 961.9°C, respectively. Without using the eutectic composition, the HMP:LMP ratio of the overall
183
184
Chapter Four Cap wafer UBM (Ti/Cu/Ni/Au)~1 μm Ag 4 μm In 2 μm Ag 0.1 μm Ag 0.1 μm In 2 μm Ag 4 μm UBM (Ti/Cu/Ni/Au)~1 μm Substrate wafer
FIGURE 4-10 The intermediate bonding layers on both sides of a bonding pair of wafers, where the schematic drawing shows the thin silver coating of both sides arranged face-to-face.
intermediate bonding layer (IBL) is selected to be high enough that the LMP component is essentially depleted into the HMP layer and reacted into high-melting-temperature IMCs. Figure 4-10 shows the IBL combination on both bonding surfaces of a pair of 8-in wafers. The IBLs include 2-μm In and 4-μm Ag layers, which are evaporated and patterned using the lift-off process on the top of the Si device wafer coated with a 300-Å Ti, 3000-Å Cu, 5000-Å Ni, and 1000-Å Au under-bump metallization (UBM) layer. Owing to the high interdiffusion rate within the layers of the IBL, some IMCs can be formed between the noble metals and indium even at room temperature. We take advantage of this and prepare a thin Ag layer of 1000 Å on top of the In layer to form a thin layer of AgIn2 at the surface. This will prevent oxidation of In layer below when these wafers are prepared and exposed to air after chamber opening. Thus we can avoid flux treatment of the wafer surface before the wafer-bonding step, so we say that it is a fluxless process. The weight percentage of the 2-μm In layer versus the 4-μm Ag layer is 25.4 percent. From the Fig. 4-9a, this 25.4 wt% In composition implies that the homogeneous phase of the bonded interface layer will be the solid solution of α′ phase and Ag. But the actual IMC phases of the bonded interface layer strongly depend on the layer sequence, interdiffusion process, and bonding conditions. In addition to the α′ phase, more IMC phases with In of 22 wt% up to 34 wt% are expected to be seen from our experimental results. Practically, the IMC phases containing In within this weight percentage range are the γ, ζ, and β phases, where these are the stable phases in each specific temperature range from ambient up to 695°C. Again, from Fig. 4-9a, we should notice that the melting point of IMCs increases with silver content, that is, eutectic composition (144°C) < AgIn2 (166°C) < γ (300°C) < ζ (670°C) < β (695°C).
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g Bonding ring of intermediate layer
Comb electrodes Comb electrodes
Torsion bar
Mirror
Mirror plate
Electrical isolation trench
Torsion bar
Comb electrodes
Posts of electrical feed-throughs
(a)
(b)
FIGURE 4-11 (a) Schematic top-view drawing of the micromirror device. (b) SEM photograph of the fabricated micromirror with two sets of vertical comb electrodes and a torsion bar.
In order to explore the feasibility of MEMS packages based on this concept, we developed an integrated process flow for making micromirror wafers and cap wafers. A silicon-on-insulator (SOI) wafer with a device layer of 30 μm, a buried oxide (BOX) layer of 2 μm, and a handle wafer of 690 μm was used for constructing the micromirror. Two steps of the DRIE process are carried out to pattern structures of the comb actuator and mirrors from the front side and to open the backside cavity for releasing the mirrors, respectively. Figure 4-11 shows a schematic drawing and scanning electron microscope (SEM) photograph of the micromirror device, respectively. The center white area represents the reflection mirror. After the backside cavity of the mirror wafer is sealed by bonding with another wafer on the backside, a dry film of photoresist is attached and lithographed on top of the mirror wafer. The In/Ag IBL is prepared by evaporation and lift-off steps. Finally, the whole mirror device is enclosed in an In/Ag IBL ring. The same In/Ag IBL ring is prepared separately on cap wafers containing a glass wafer on a silicon wafer with through-wafer holes. During the bonding process, these wafers are aligned and put into a bonding chamber under 6 mtorr of pressure first. Then the fluxless solder bonding is conducted at 180°C for 40 minutes under 8 kN of applied bonding force. Both the hermetically sealed ring and the electrical interconnects are formed at this bonding step. As shown in Fig. 4-11a, two metal posts on the mirror chip are separated electrically by a silicon trench. These two metal posts are connected electrically via a metal line on the cap-wafer side. The metal posts cross underneath the solder sealing ring with dielectriclayer passivation. Thus the hermetic sealing can be kept inside the sealed cavity. Figure 4-12a shows a top view of the bonded 8-in wafers. Figure 4-12b shows the wafer-bonding-packaged micromirror chip after dicing, whereas Fig. 4-12c shows an x-ray image of the bonded
185
186
Chapter Four
(a)
(c)
(b)
(d)
FIGURE 4-12 (a) The bonded 8-in-diameter stack wafers. (b) Top-view photograph of separated micromirror chip with the reflective mirror at the center. (c) X-ray image of one chip area of cap wafer with bonding ring shown in dark square ring pattern. (d ) Photograph of diced micromirror chip after assembly on a DIP carrier.
wafer is taken from the cap-wafer side. The bright square in the center of micromirror chip in Fig. 4-12b is the reflective micromirror. Then the wafer-bonding-packaged micromirror chip is assembled on a dual in-line package (DIP) carrier for further device function testing, as shown in Fig. 4-12d.
Effect of Postbonding Annealing First, we conducted the postbonding annealing at 130°C for 24 hours for the wafer-bonding-packaged mirror chips after dicing in an N2filled furnace. Properly diced chips were mounted on epoxy resin and subsequently polished. The cross-sectional elemental composition of the bonded interface was characterized by energy dispersive x-ray spectroscopy (EDX). Samples were mounted on epoxy resin and subsequently polished. Figure 4-13 shows the weight percentage of all the components as a function of the depth along the bonded interface. Along the cross section of the bonded interface it is observed
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g 100 90
Weight percentage, %
80 70 Ag In Ti Ni cu
60 50 40 30 20 10 0
0
1
2
3
4
5 6 7 8 9 10 11 12 13 14 15 Interface thickness, μm
FIGURE 4-13 EDX analysis data along a cross section of the bonded interface.
that there is an intermediate layer of a homogeneous composition with a thickness of about 7.5 μm at the center zone. The composition ratio of this intermediate layer is referred to as the Ag9In4 IMC phase mainly, whereas the IMC phase at 7 μm is called the Ag2In phase because both Ag2In and Ag9In4 are the observed phases based on crystal structure analysis by XRD for the samples bonded at 180°C.67 It also should be noticed that there is a thin pure Ag layer of about 1 μm thickness on both sides of the IBL. These two pure Ag layers are referred to the remaining Ag on top of the UBM layers on the two bonding wafers. It also means that the current IBL design leads to IMCs with high remelting temperatures (e.g., γ of 300°C and ζ of 670°C). In other words, the HMP:LMP ratio of the IBL in Fig. 4-10 is an appropriate combination. The bonded interface of Ag9In4 and/or Ag2In IMC phases and pure Ag will guarantee a MEMS package with good high-temperature resistance to postbonding process temperatures (e.g., SMT peak temperature of 285°C).
Effect of Long-Term Room-Temperature Storage It has been reported that Ag2In and AgIn2 are the stable phases at temperatures above and below 100°C in an In-Ag diffusion-couple experiment using thick foils of pure In and Ag.68 When the diffusion couple with a dominant IMC of Ag2In was cooled down and maintained at room temperature for a long time, the Ag atoms diffused from some Ag2In grains into the adjacent pure Ag grains, and In atoms from adjacent pure In grains diffused into the Ag2In grains.
187
188
Chapter Four Some of these Ag2In grains gradually became AgIn2 grains. In a later stage, the grain boundary of these AgIn2 grains expanded continuously by consuming adjacent Ag2In grains (i.e., the grain-growth process). Eventually, AgIn2 became the major IMC phase along the interface of the diffusion couple after room-temperature storage for a long time (e.g., 1 month).68 Because of this, we have kept diced chips in N2-filled containers at room temperature for 80 days (the chips were derived from bonded wafers that were bonded at 180°C for 40 minutes). We investigated the bonded interfaces of these chips via EDX analysis. Figure 4-14a shows a SEM photograph of the bonding-interface cross section denoted along with the phase composition, whereas the Fig. 4-14b shows the measured EDX results, which are plotted versus the position of bonding interface. In addition, the original positions of all layers except the UBM are marked on the left side of Fig. 4-14a. Figure 4-14c and d shows the results from another chip. First, no pure In phase is observed. We also concluded that both Ag2In and AgIn2 coexist in the bonding interface after room-temperature storage of 80 days. Some data points are derived with a weight percentage close to that of Ag9In4, as shown in Fig. 4-14c. For example, the composition at 3.3 μm in Fig. 4-14d is matched with Ag9In4. This observation is in agreement with previous bulk-based diffusion-couple results.68
Effect of Aging When we consider the postdicing chip-assembly process, such a process typically involves baking of the solvent and/or curing at low temperature. In the case of a packaged MEMS devices used in some high-temperature environment, the question becomes, What is the influence of such aging treatment? Thus we have kept diced chips in an N2-filled container at 70°C for 80 hours (where these chips have been stored at room temperature for 80 days and were derived from a bonded wafer that was bonded at 180°C for 40 minutes). The EDX results of a cross section of the bonded interface are shown in Fig. 4-15. We have conducted several line-scan analyses. Two of these line-scan data results are plotted in Fig. 4-15b and c. These data consistently show that the amount of AgIn2 phase is increasing when we compare these samples with long-term room-temperature storage samples and the as-bonded samples. However, the bonding interface does not convert into single IMC AgIn2 phase after this aging at 70°C for 80 hours. Given that the original weight ratio of Ag/In in the present IBL combination is 2.94, we strongly believe that the single IMC phase of AgIn2 will never happen at the bonding interface even after an extremely long period of low-temperature aging. The melting temperature of AgIn2 is 166°C. Thus the existing AgIn2 may be a concern in terms of long-term reliability.
Effect of Additional Postbonding Annealing In the last part of the experiment, we explored the influence of annealing. We have kept diced chips in an N2-filled container at 120°C for 80 hours
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g
Mixture of Ag2In and AgIn2
Ag
Mainly Ag2 In
In Ag In
Mainly AgIn2
Ag
(a) 100 In
Ag
Weight %
80 60 40 20 0
(b)
0
2
4
6
8
12
10
Position along cross section of the bonded interface (μm)
AgIn2 Mixture of AgIn2 and Ag2In Ag9In4 Mixture of AgIn2 and Ag2In
Ag In Ag In
Ag2In/Ag9In4
Ag AgIn2
(c) 100 Ag
In
Weight %
80 60 40 20 0
(d)
0
2
4
6
8
10
12
Position along cross section of the bonded interface (μm)
FIGURE 4-14 Study of the bonded interface after long-term room-temperature storage: (a) SEM photograph of first chip with the identified IMC phases denoted; (b) EDX data derived from the spots shown in part a; (c) SEM photograph of the second chip denoted with the identified IMC phases denoted; (d ) EDX data derived from the spots shown in part c.
189
190
Chapter Four
A
B
Ag AgIn2
AgIn2 In Ag In
Mixture of Ag2In and AgIn2
Ag
Mixture of Ag2In and AgIn2 Ag
(a) 100
Weight %
Ag
A scan
80
In
60 40 20 0
0
2
4
6
8
10
12
Position along cross section of the bonded interface (μm)
(b) 100
B scan Weight %
80 Ag
In
60 40 20 0
(c)
0
2
4
6
8
10
12
Position along cross section of the bonded interface (μm)
FIGURE 4-15 Study of the bonded interface under low-temperature aging: (a) SEM photograph showing the identified IMC phases; (b) EDX data derived from scan-line A in part a; (c) EDX data derived from scan-line B in part a.
(and these chips have been stored at room temperature for 80 days and were derived from a bonded wafer that was bonded at 180°C for 40 minutes). The SEM photograph and line-scan-based EDX results of the cross section of the bonded interface are shown in Fig. 4-16. Interestingly, single-phase IMC of Ag2In has been observed and occupies the major portion of the bonding interface. Compared with the case in Fig. 4-13 (i.e., with existing pure Ag phase on both sides), Fig. 4-16 shows very limited thickness of the remaining phase other than Ag2In.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g
A
B
Ag In Ag In
Ag2In
Ag
Ag2In
Mixture of Ag, In, Ti, and Ni
Mixture of Ag, In, Ti, and Ni
(a) 100 Ag
A scan
In
Weight %
80 60 40 20 0
0
(b)
2
4
6
8
10
12
Position along cross section of the bonded interface (μm) 100
Weight %
Ag
B scan
80
In
60 40 20 0
(c)
0
2
4
6
8
10
12
Position along cross section of the bonded interface (μm)
FIGURE 4-16 Study of bonded interface under additional annealing effect: (a) SEM photograph with identified IMC phases denoted; (b) EDX data derived from scan-line A shown in part a; (c) EDX data derived from scan-line B in part a.
This result points out that appropriate low-temperature annealing (e.g., at 120°C for 80 hours) can effectively get rid of low-meltingtemperature IMC phases, that is, AgIn2. In particular, the composition at the 2-μm position of the scan in Fig. 4-16a is quite close to Ag9In4. We can imagine that such annealing at 120°C for 80 hours could be well accepted by most packaged MEMS devices. Thus we can apply this annealing step to refine the microstructure of the sealing rings of packaged MEMS devices.
191
192
Chapter Four
Ag wt%
In wt%
100.00
0
100.00
0
70.77
29.23
71.39
28.61
68.07
31.93
69.38
30.62
65.11
34.89
67.6
32.40
69.68
30.32
67.53
32.47
100.00
0
Cu Ti, Ni, and Cu Ag
Ag
In Ag In
Ag2In/Ag9In4
Ag Ag Ni, Ag, and Cu
10 μm
FIGURE 4-17 SEM photograph of the bonded interface after prolonged additional annealing. EDX results are shown on left side, and the suggested IMC phases are shown on right side.
On the other hand, some microcracks are observed at the bonding interface for the samples that underwent an even longer annealing step (i.e., 120 hours at 120°C). Figure 4-17 shows that the dominant phases are Ag2In and Ag9In4, whereas microcracks appear at the bonded interface. Both Ag2In and Ag9In4 are the high-melting-temperature phases and are desired to be the final IMCs at the interface. Moreover, to explore the reason behind such microcracks, we first calculate the density of AgIn2 as 8.43 g/cm3 and the density of Ag2In as 9.78 g/cm3. Then we determined the corresponding volume change of AgIn2 in unit mass to Ag2In in unit mass as an increment of 13.8 percent. The IBL ring structure is confined between two substrates and cannot absorb 13.8 percent volume expansion easily. Thus the residual stress eventually leads to the observed microcracks. A meander trace on the IBL ring and a narrow ring may be potential ways to release the residual stress so as to avoid microcrack generation. High-melting-temperature IMCs of Ag9In4 and Ag2In at the interface are derived after additional annealing at 120°C for 80 hours for samples after long-term room-temperature storage. The melting temperature of IMCs of Ag9In4 and Ag2In is higher than 400°C. This implies that appropriate annealing can get rid of low-melting-temperature IMC phases (e.g., AgIn2). However, prolonged annealing in this situation leads to the generation of microcracks because the IBL ring faces a significant volume change from phase transformation (i.e., from AgIn2 into Ag2In).
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g
4.5.2
Case Study: Eutectic InSn Solder for Cu-Based Metallization
In order to obtain a high yield of good bonded dies via wafer bonding, issues of wafer warpage and topography differences along the bonding rings across a wafer can be overcome by a solder-reflow step when sufficient solder is placed in the bonding rings. However, the LMP solder has to be fully consumed by reacting with HMP metals during the bonding and annealing steps to form reliable and hightemperature-resistant IMC phases at the bonding rings for hermetic sealing applications. This suggests that solder layers of reasonable thickness are an important case-sensitive parameter. We have studied the interface microstructure of Sn/In/Au/Cu metallization after solder deposition in detail. Since the diffusion rates between low-temperature solders and HMP metal substrates such as Cu and Au are very high, a portion of the as-deposited solders on the HMP metal would be consumed before the wafer-bonding step. As shown in Fig. 4-18, it is obvious that extensive interdiffusion between
InSn
AuIn2
Cu6(Sn,In)5
Cu
1 μm
1 μm
FIGURE 4-18 TEM analysis of thin Au0.03/(InSn)3/Au0.03/Cu2 metallization after deposition (thickness in microns). In order to accelerate the interdiffusion between Sn and In and to obtain an In-Sn alloy before bonding, 10 thin alternative In/Sn solder layers with each layer 0.3 µm thick were deposited by E-beam evaporation. The Au layers were deposited to protect the Cu and solder from getting oxidized.
193
194
Chapter Four solder materials (i.e., Sn and In) and Au/Cu layers occurs. On the Cu substrate, Cu6(Sn, In)5 ternary phase was formed owing to interdiffusion. Additionally, Au diffused toward the solder side to from the AuIn phase, which was found inside the Cu6(Sn, In)5 phase. The residual low-temperature SnIn phase is located at the top of the interface, as shown by the dashed line in the figure. Based on preliminary 8-in wafer-bonding results using these SnIn/Au/Cu layers, complete depletion of the low-temperature solders in the as-deposited films would lead to a low yield of good bonded dies.69,70 Owing to the lack of reflow function provided by low-temperature solders, large voids and cracks were found inside the joint, and the hermeticity was quite poor. We screened the bonded dies after dicing by using cross-sectional scanning acoustic microscopy (C-SAM). A die was labeled as a “good die” if there were no detectable voids and/or cracks under C-SAM. The bonding yield was further defined as the percentage of “good dies” to the “bad dies” of a bonded wafer. As listed in Table 4-3, the bonding yield was 44 and 67 percent with a pressure of 3 and 5.5 MPa at 180°C for 20 minutes. Limited improvement was observed when the bonding pressure was increased.70 Therefore, prevention of interdiffusion between LMP and HMP components during the fabrication process and room-temperature storage is the key to obtaining high-yield wafer-to-wafer bonding. As described in Fig. 4-19, a thin buffer layer is introduced in between the Cu substrate and the solder layers such that interdiffusion is inhibited, whereas this thin buffer layer preferentially dissolves into the melted solder quickly at the beginning of soldering reaction (see Fig. 4-19b and c). Then the diffusion between the liquid solder and the Cu starts, and finally, all solder was converted into IMCs (see Fig. 4-19d). Since the buffer layer saves the low-temperature materials for a successful solder-reflow step during bonding, the production yield of wafer bonding is improved significantly. Ni is well known as a barrier layer for Sn-based solder and Cu substrate, and at the same time, it can easily diffuse into Cu-based IMCs.71 Thus a thin Ni buffer layer was chosen and investigated to control diffusion mechanism between In-Sn solder and Cu. For In/Sn/Cu systems after eutectic bonding, we hope that all low-temperature phase can be converted to high-temperature IMCs. According to the ternary-phase diagram of Cu-In-Sn, the calculated thickness ratio of Cu to In-Sn needs to be larger than 0.5 to form Cu6(Sn, In)5 compounds. To protect In-Sn from oxidization, a thin Au layer is deposited on top of the solder layers. Since In will form Au-In IMCs with Au, there will be two kinds of IMCs in the final seal joint: Cu6(Sn, In)5 and Au-In. To get a robust joint, the Au layer should be as thin as possible to reduce the volume of the Au-In IMC. To validate this new combination of materials for wafer bonding, we conducted a wafer-bonding experiment. First, 300-Å-thick SiO2 and 1500-Å-thick SiN were formed on a silicon wafer by thermal oxidation
Cap Wafer (Thickness in Micron) Wafer Pair 1 2
HMP Component Cu2/Au0.03 Cu2/Au0.03
Solder (Sn/In)3∗ (Sn/In)3∗
Bottom Wafer (Thickness in Micron) HMP Component Cu2/Au0.03 Cu2/Au0.03
Bonding Parameter Pressure (MPa)
Temperature (∞C)
Time (min)
Yield (%)
†
3.0
180
20
44
†
5.5
180
20
67
Solder (Sn/In)4
(Sn/In)4
∗Ten layers in turn, each layer was 0.3 μm. † Ten layers in turn, each layer 0.4 μm.
TABLE 4-3 Bonding Experiments of In-Sn Low-Temperature Solders versus Cu Bonding Rings
195
196
Chapter Four • Buffer layer Copper Copper
Copper
Liquid solder
Liquid solder
Copper
Copper
Solder • Au Solder Copper (a)
(b)
(c)
IMCs
(d)
FIGURE 4-19 Schematic drawing of the role of a buffer layer during bonding: (a) before bonding; (b) liquid solder formed at the beginning of wafer bonding; (c) buffer layer dissolved into solder; (d ) high-temperature IMC joint finally formed during bonding.
and the LPCVD process. They acted as a photolithography mask for cavity etching. A cavity with a 6 × 6 mm2 area and 250-μm depth was formed using a KOH wet-etching process inside each bonding ring on both the cap wafer and the bottom wafer. By using photolithography to pattern dry film as a lift-off mask, Ti/Cu/Ni/Au metallization was sputtered on Si/SiO2/SiN substrate as the HMP component for diffusion bonding. The thickness of Ti/Cu/Ni/Au metallization was designed as 0.05, 2, 0.05, and 0.03 μm, respectively. The multilayered bonding-ring structure is shown in Fig. 4-20. The thin Ti layer acting as the adhesive layer is not shown in the figure, and the Ni is the buffer layer. We used the well-known Ti/Cu/Ni/Au under-bump metallization (UBM) process to prepare the HMP component while we increased the thickness of Cu layer up to 2 μm. Thus we called these HMP rings UBM rings. Then the solder layers and Au protection layer were deposited in turn in an E-beam evaporation chamber. After another dry-film-strip step, 300-μm-wide square bonding rings 11 mm long were finally fabricated on a wafer with
Au In Sn Ni Cu
FIGURE 4-20 Schematic depiction of the InSn solder versus Ti/Cu/Ni/Au UBM metallization.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g cavities. After deposition and dry-film stripping, O2 plasma descum was conducted before the bonding process to remove the oxide layer and organic contaminants to produce a clean surface. In the waferbonding step, two wafers with cavities enclosed by bonding rings were aligned and brought into the vacuum chamber of a commercial wafer bonder. When the wafers were heated up to 180°C (i.e., bonding temperature), a bonding pressure of 5.5 MPa was applied to press the bonding-pair wafers into tight contact for 20 minutes. After the bonding step, the wafer was diced into chips of 13 × 13 mm2 in which each chip has a vacuum cavity sealed inside the bonded structure (Fig. 4-21). Scanning acoustic microscopy (SAM) was deployed for nondestructive study of the bonding interface. There were no detectable voids in any single seal ring. This meant that a 100 percent yield after bonding was achieved by this bonding method. A typical C-SAM graphs of dies is shown in Fig. 4-22.
FIGURE 4-21 Photo of a successfully bonded wafer with 100 percent yield.
FIGURE 4-22 SAM graph of bonded devices using Ti/Cu/Ni/Au UBM. The bonding temperature was 180°C.
197
198
Chapter Four Each bonding ring was a uniform gray color, indicating the bonded joints have intimate contact. The hermeticity of the ring seals for pattered dies was evaluated by helium leak-rate testing (MIL-STD-883). A shear test was done with a shear tester (BT4000 Dage) using a speed of 50 μm/s. Reliability tests of the bonded devices was studied in detail. A pressure-cooker test was conducted at 121°C and 2 atm for 300 hours. High-humidity storage was done at 85°C and 85 percent relative humidity (RH) for 1000 hours. A high-temperature storage test at 125°C and a temperature cycling test (–45 to 125°C) for up to 1000 hours also were performed. For each item, 21 chips were tested. After the tests, these chips were examined by SAM and helium leak-rate and shear tests again.
Reliability Study The microstructure of the bonded interface is shown in Fig. 4-23 in the case of 180°C bonding. In the center region of the bonded interface, thick residual Cu and a thin IMC layer were found, as shown in the figure. Two kinds of IMCs were detected by EDX. One composition (atomic percent) is Cu:Ni:In:Sn = 56.17:4.63:12.37:26.84, which also corresponds to the η phase, that is, (Cu, Ni)6(Sn, In)5. Another is AuIn2 phases with white-particle morphology. According to the present materials design, the thickness of the seal joint should be around 10 μm. However, the actual thickness value achieved was about 7 μm. Under the present bonding temperature, solder materials melt fast and have good flowability. When bonding pressure was applied, a portion of the liquid alloy squeezed out. As shown in Fig. 4-23b, the length of the squeezed solder was about 80 μm. In order to know the kinetics of the bonding process involving the Ni buffer layer, TEM/EDX analysis was performed on the seal joint. The results are shown in Fig. 4-24 and Table 4-4. It was found that the
Au(In, Sn)2 Cu
Cu
Squeezed solder (Cu, Ni)6(Sn, In)5
(a)
(b)
FIGURE 4-23 Interfacial microstructure of the joint bonding at 180°C: (a) center region of the joint; (b) bonded joint of two wafers.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g
0.5 μm
FIGURE 4-24 TEM/EDX analysis of the seal-ring joint after bonding. In order to find the trace of the Ni buffer layer, the analyzing position is near the residual Cu.
Element (at%) Position
Cu
1
88.1
2
47.4
3
32.6
8
4
36.5
11.7
5
5.7
6
11.6
7
42.6
TABLE 4-4
Ni 4.8
6
Sn
In
7.1
4.8
35.4
17.2
43.2
16.2
Au
45
6.8
6
55.1
33.3
13.2
47.6
27.7
41.8
9.6
Compositions of Selected Positions of TEM/EDX
Analysis
phase adjacent to the Cu substrate was Cu6(Sn, In)5, and next was (Cu,Ni)6(Sn, In)5. Island shape Au(In, Sn)2 phases embedded in the (Cu, Ni)6(Sn, In)5 phase also were identified. These results confirmed that the Ni buffer layer had been dissolved into a Cu6(Sn, In)5 IMC and formed a (Cu, Ni)6(Sn, In)5 phase in some regions. The content of Ni in this quaternary phase can reach 11.7 at%. The bonding process involving the buffer layer can be explained as follows: First, owing to the slow reaction between solder and Ni at room temperature, a major portion of the solder remains on top of the Ni
199
200
Chapter Four buffer layer. When wafers are heated up to the bonding temperature, the solder melted and started to react with the thin Ni buffer layer. The Ni dissolved into the solder as Ni3Sn4 or NiInSn ternary phase72,73 according to studies of the interfacial reactions between liquid InSn solder and Ni. Since the Ni buffer layer is very thin, after a short time, InSn solder started to react with Cu to form Cu6(Sn, In)5 compounds. Since Ni has great solubility in the Cu6(Sn, In)5 compounds, a chemical potential gradient was generated, which led to dissolution of the Ni-containing compounds. Finally, all Ni atoms went into Cu6(Sn, In)5 solution to form the (Cu, Ni)6(Sn, In)5 phase. The testing results showed that the leak rates of all the samples bonded at 180°C were less than 5 × 10–8 (atm · cc)/s, which indicated that the dies obtained acceptable hermeticity based on the criteria of MIL-STD-883. The average shear strength of the joints was 32.13 MPa, which meant that robust bonding strength was achieved for these patterned dies. These results indicate that the Ni buffer layer plays an important role in achieving high-yield wafer-level hermetic bonding. The results of the reliability tests show that ratios of dies with a leak rate of less than 5 × 10–8 (atm · cc)/s after the pressure-cooker test, high-humidity storage, high-temperature storage, and temperature cycling were 71.4, 90.5, 76.2, and 81 percent, respectively. Meanwhile, the tested chips still maintain good mechanical properties. The shear test after pressure cooker test, high humidity storage, high temperature storage and temperature cycling were 27.08, 15.37, 12.32, 16.71 MPa, respectively. As shown in Fig. 4-25, the interfacial microstructures were analyzed after the reliability tests as well. The results show that embedded AuIn compounds congregated and that the size of the accumulation became larger at the interface. With further EDX analysis, the compositions of the bonding interface do not show any detectable change. Such results are reasonable because the temperatures for the reliability tests was not high enough to introduce phase changes at the IMC joints. However, based on the shear-test results, we believe that the adhesion between different IMCs decreased after reliability testing. Bonded chips with poor hermeticity were analyzed to know the failure mechanism of the bonding interface after reliability testing. As shown in Fig. 4-26, visible cracks throughout the bonding interface were found in these samples with poor leak-rate test results. It is clear that the crack expanded along the interface between AuInSn compounds and CuSnIn compounds. Stress generated at the interface between different IMCs when bonded chips were tested under thermal cycling and the pressure-cooker test. This is the reason why after these two tests, the leak-rate test revealed a relative poor hermeticity results compared with other tests. This implies that the adhesion between the two IMC phases is the key to determining the reliability of the bonded chips. Two ways are proposed to improve reliability further. The first is to reduce the amount of AuInSn compound
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g
(a)
(b)
(c)
(d)
FIGURE 4-25 Interfacial microstructure of the seal joints of good dies after reliability tests: (a) high-temperature storage; (b) temperature cycling; (c) high-humidity storage; (d ) pressure-cooker test.
(a)
(b)
FIGURE 4-26 Cracks along the interface after reliability tests: (a) temperature cycling; (b) pressure-cooker test.
by depositing a much thinner Au protection layer for fluxless bonding. The second approach is to increase the amount of low-temperature solder. As a result, the potential to form a continuous Au-rich IMC phase at the interface is reduced significantly. In this way, the reliability of the bonded interface can be improved.
201
202
Chapter Four Low-cost and high-yield wafer-to-wafer bonding using In/Sn solder and a Cu/Ni/Au metallization system was investigated, and the process produced successful bonding at 180°C. Various tests were conducted to evaluate the reliability of the bonded devices. Cracks formed at the interface of the bonded chips after reliability testing are the main cause of deterioration of the bonded interface.
4.6
Summary and Future Outlook After a decade of research and commercialization, wafer-level packaging has proven to be a leading solution for MEMS packaging. In addition to the package size, cost, and performance advantages, wafer-level MEMS packaging provides a way for enabling a SiP-type of ultracompact and thin hybrid package that integrates MEMS, optoelectronics, signal-processing circuits, and even energy sources. In addition to the wafer-bonding type of MEMS packaging based on a BCB intermediate layer, a low-cost, near-hermetic package using a liquid-crystal polymer (LCP) substrate, cap, and sealing ring has been deployed widely for packaging CMOS image sensors nowadays. LCP is a thermoplastic polymer with barrier properties that are an order of magnitude greater than those of epoxy plastic materials. The permeability of LCP to water vapor and oxygen is close to that of glass. Without using wafers containing etched cavities, a thick LCP ring can be used as the necessary spacing layer between two bonded wafers that provides enough room for the motion of MEMS moving parts. A sealed LCP cavity can pass helium leak-rate testing (i.e., MILSTD-883E). However, this sort of testing may not be appropriate for polymer-type packages because it measures only fine and gross leaks without considering permeability and outgassing. Although LCPand BCB-based MEMS packages cannot be considered to be hermetic packages, they could be a cost-effective MEMS packaging solutions for consumer electronics applications. Some of MEMS devices require a controlled atmosphere in the cavity or even a vacuum-packaged cavity. Low-temperature-solderbased wafer bonding can be an effective and low-cost approach to enabling vacuum-packaged MEMS devices. The eutectic InSn solder versus Cu/Ni/Au UBM is characterized as a promising bonding-ring material combination. Wafer-level packaging of vacuum cavities brings the cost advantage of permitting simultaneous sealing of an entire wafer of cavities in a vacuum. This eliminates the manufacturing inefficiencies and costs involved in individual “pump down and pinch off” for archaic conventional metal or ceramic vacuum packages. Wafer-level packaging based on direct bonding, metal-intermediatelayer bonding, and metal-sealed encapsulation may provide the lowcost MEMS vacuum packaging solutions of the future. However, if we want to maintain the high vacuum over long lifetimes, the materials
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g and seals used must be leak-free, impermeable, and not sources of significant outgassing. The high surface-to-volume ratio of these microcavities makes the maintenance of packaged vacuum even more difficult in wafer-level MEMS packaging. These surfaces are reservoirs of adsorbed gases such as oxygen, carbon dioxide, and reactive gases. A plated metal surface is considered a major source of dissolved hydrogen, which is a potential device killer in some cases. Integrating getter film into the packaged cavities may be a good solution to overcome these concerns for enabling wafer-level MEMS vacuum packaging.33,74 On the other hand, the conventional standard of hermeticity based on MIL-STD-883E is invalid for cavity volumes of less than 1000 nl3. Currently, people measure wafer-level vacuumpackaged MEMS device characteristics and calibrate the measured data with data derived for devices tested in a well-controlled vacuum chamber with a known degree of vacuum. A MEMS resonator can allow us to discriminate the degree of vacuum from 0.1 torr to several tens of torrs.75 A Pirani sensor or a resistive type of thermal sensor with a suspended membrane structure on a V-groove may allow us to measure the degree of vacuum from ambient down to 0.1 torr,76 whereas a degree of vacuum of 4 mtorr can be detected using a bolometer or a resistive type of thermal sensor on the surfacemicromachined membrane with tight gap between the suspended membrane and substrate.77 It is also reported that Pirani sensors using proper readout circuits to counter the self-heating effect can allow us to measure the degree of vacuum down to 10–7 torr.78 However, more research effort is needed to establish the external wafer-level nondestructive characterization approaches for MEMS wafer-level vacuum packaging. Thus we may increase the testing speed and reduce cost.
References 1. Williams, K. R., and Muller, R. S. “Etch rates for micromachining processing.” J. Microelectromech. Syst. 5:256–269, 1996. 2. Petersen, K. E. “Silicon as a mechanical material.” Proc. IEEE 70:420–457, 1982. 3. Hoffmann, E., Warneke, B., Kruglick, E., Weigold, J., and Pister, K.S.J. “3D structures with piezoresistive sensors in standard CMOS.” In Proceedings of the IEEE Microelectromechanical Systems, Amsterdam, The Netherlands, January 29–February 2, 1995, pp. 288–293. 4. Tabata, O. “pH-controlled TMAH etchants for silicon micromachining.” Sensors & Actuators A53:335–339, 1996. 5. Klaassen, E., et al. “Micromachined thermally isolated circuits.” In Proceedings of the 1996 Solid-State Sensor and Actuator Workshop, Hilton Head Island, SC, June 3–6, 1996, pp. 127–131. 6. Moser, D. “CMOS flow sensors.” Ph.D. dissertation, Swiss Federal Institute of Technology, Zurich, Switzerland, 1993. 7. Seidel, H. “The mechanism of anistotropic silicon etching and its relevance for micromachining.” In Proceedings of Transducers ‘87, Record of the 4th International Conference on Solid-State Sensors and Actuators, Tokyo, Japan, June 2–5, 1987, pp. 120–125.
203
204
Chapter Four 8. Seidel, H., Csepregi, L., Heuberger, A., and Baumgärtel, H. “Anisotropic etching of crystalline silicon in alkaline solutions: I. Orientation dependence and behavior of passivation layers.” J. Electrochem. Soc. 137:3612–3626, 1990. 9. Abe, H., Yoneda M., and Fujiwara, N. “Developments of plasma etching technology for fabricating semiconductor devices,” Jpn. J. Applied Physics, 47: 1435–1455, 2008. 10. Lärmer, F., and Schlip, P. “Method of anisotropically etching silicon,” German Patent No. DE 4,241,045, 1994. 11. Chang, F. I., Yeh, R., Lin, G., Chu, P. B., Hoffman, E., Kruglick, E. J., Pister, K. S. J., and Hecht, M. H. “Gas-phase silicon micromachining with xenon difluoride.” In Proceedings of SPIE: Microelectronic Structures and Microelectromechanical Devices for Optical Processing and Multimedia Applications, Austin, TX, July 1995, Vol. 2641, pp. 117–128. 12. Schmidt, M. A. “Wafer-to-wafer bonding for microstructure formation.” Proc. IEEE 86:1575–1585, 1998. 13. Shimbo, M., Furukawa, K., Fukuda, K., and Tanzawa, K. “Silicon-to-silicon direct bonding method.” J. Appl. Phys. 60:2987–2989, 1986. 14. Kanda, Y., Matsuda, K., Murayama, C., and Sugaya, J. “The mechanism of field-assisted silicon-glass bonding.” Sensors & Actuators A21–A23:939, 1990. 15. Wolffenbuttel, R. F., and Wise, K. D. “Low-temperature silicon wafer-to-wafer bonding using gold at eutectic temperature.” Sens. Actuators A 43:223–229, 1994. 16. Sparks, D., Massoud-Ansari, S., and Najafi, N. “Long-term evaluation of hermetically glass frit sealed silicon to Pyrex wafers with feedthroughs.” J. Micromech. Microeng. 15:1560–1564, 2005. 17. Kim, W., Wang, Q., Jung, K., Hwang, J., and Moon, C. “Application of Au-Sn eutectic bonding in hermetic rf MEMS wafer level packaging.” In Proceedings of the 9th International Symposium on Advanced Packaging Materials: Processes, Properties and Interfaces, Atlanta, Georgia, March 24–26, 2004, pp. 215–219. 18. Shiv, L., Heschel, M., Korth, H., Weichel, S., Hauffe, R., Kilian, A., Semak, B., Houlberg, M., Egginton, P., Hase, A., and Kuhmann, J. “Ultra thin hermetic wafer level, chip scale package.” In IEEE Proceedings of the Electronic Components & Technology Conference (ECTC 2006), San Diego, CA, May 30–June 2, 2006, pp. 1122–1128. 19. Niklaus, F., Stemme, G., and Gutmann, J.-Q., R. J. “Adhesive wafer bonding.” J. Appl. Phys. 99:31101, 2006. 20. Jourdain, A., DeMoor, P., Baert, K., De Wolf, I., and Tilmans, H. A. C. “Mechanical and electrical characterization of BCB as a bond and seal material for cavities housing rf-MEMS devices.” J. Micromech. Microeng. 15:S89–S96, 2005. 21. Lin, C.-H., Lu, J.-M., and Fang, W. “Encapsulation of film bulk acoustic resonator filters using a wafer-level microcap array.” J. Micromech. Microeng. 15:1433– 1438, 2005. 22. Satyanrayana, s., Karnik, R. N., and Majumdar, A. “Stamp-and-stick roomtemperature bonding technique for microdevices.” J. MEMS 14:392–399, 2005. 23. Oberhammer, J., and Stemme, G. “BCB contact printing for patterned adhesive full-wafer bonded 0-level packages.” J. MEMS 14:419–425, 2005. 24. Weinert, A., Amirfeiz, P., and Bengtsson, S. “Plasma assisted room temperature bonding for MST.” Sensors & Actuators A 92:214–222, 2001. 25. Dragoi, V., Mittendorfer, G., Thanner, C., and Lindner, P. “Wafer-level plasma activated bonding: New technology for MEMS fabrication.” Microsyst. Technol. 14:509–515, 2008. 26. Takagi, H., Kikuchi, K., Maeda, R., Chung, T. R., and Suga, T. “Surface activated bonding of silicon wafers at room temperature.” Appl. Phys. Lett. 68:2222–2224, 1996. 27. Takagi, H., Maeda, R., and Suga, T. “Wafer-scale room-temperature bonding between silicon and ceramic wafers by means of argon-beam surface activation.” In Proceedings of the IEEE Workshop on MEMS, Interlaken, Switzerland, January 21–25, 2001, pp. 60–63. 28. www.hymite.com/.
A d v a n c e d M E M S Wa f e r- L e v e l P a c k a g i n g 29. Kuhmann, J. F., Heschel, M., Bouwstra, S., Baleras, F., and Massit, C. “Through wafer interconnects and flip-chip bonding: A toolbox for advanced hybrid technologies for MEMS.” In Proceedings of the 13th European Conference on Solid-State Transducers, Eurosensors The Hague, The Netherlands, September 12–15, 1999, pp. 265–272. 30. Takizawa, T., et al. “Conductive interconnections through thick silicon substrates for 3D packaging.” In Proceedings of the IEEE 15th International Conference on MEMS, Las Vegas, NV, January 20–24, 2002, pp. 388–391. 31. Satoh, A. “Mechanism and characteristics of through-holes formation on silicon wafer by optical excitation electropolishing method.” Jpn. J. Appl. Phys. 39:1612–1621, 2000. 32. Wang, Z., Wang, L., Nguyen, N. T., Wien, W. A. H., Schellevis, H., Sarro, P. M., and Burghartz, J. N. “Silicon micromachining of high aspect ratio, high-density trough-wafer electrical interconnects for 3D multichip packaging.” IEEE Trans. Adv. Packag. 29:615–622, 2006. 33. Premachandran, C. S., Chong, S. C., Liw, S., and Nagarajan, R. “Design, fabrication and testing of wafer level vacuum package for MEMS device.” In IEEE Proceedings of the Electronic Components & Technology Conference, San Diego, CA, May 30-June 2, 2006, pp. 1136–1140. 34. Park, J.-H., Lee, H.-C., Park, Y.-H., Kim, Y.-D., Ji, C.-H., Bu, J., and Nam, H.-J. “A fully wafer-level packaged rf MEMS switch with low actuation voltage using a piezoelectric actuator.” J. Micromech. Microeng. 16:2281–2286, 2006. 35. Ho, S. W., Rao, V. S., Khan, O. K. N., Yoon, S. U., and Kripesh, V. “Development of coaxial shield via in silicon carrier for high frequency application.” In IEEE Proceedings of the Electronic Packaging & Technology Conference, San Diego, CA, May 30-June 2, 2006, pp. 1–6. 36. Matijasevic, G. S., Lee, C. C., and Wang, C. Y. “Au-Sn alloy phase diagram and properties related to its use as a bonding medium.” Thin Solid Films 223: 276–287, 1993. 37. Wolffenbuttel, R. F., and Wise, K. D. “Low-temperature silicon wafer-to-wafer bonding using gold at eutectic temperature.” Sensors & Actuators A 43:223–229, 1994. 38. Huang, W.-F., Shie, J.-S., Lee, C., Gong, S. C., and Peng, C.-J. “Development of low-temperature wafer level vacuum packaging for microsensors.” Proc. SPIE 3893:478–485, 1999. 39. Lee, C., Shie, J.-S., and Huang, W.-F. “Wafer bonding by low temperature soldering.” Sensors & Actuators A 85:330–334, 2000. 40. Brand, O., and Baltes, H. “Microsensor packaging.” Microsyst. Technol. 7: 205–208, 2002. 41. Gooch, R., Schimert, T., McCardel, W., Ritchey, B., Gilmour, D., and Koziarz, W. “Wafer-level vacuum packaging for MEMS.” J. Vac. Sci. Technol. A 17:2295–2299, 1999. 42. Gooch, R., and Schimert, T. “Low-cost wafer-level vacuum packaging for MEMS.” MRS Bull. 28:55–59, 2003. 43. Gooch, R. “Vacuum package fabrication of MEMS devices with integrated circuit components,” U.S. Patent No. 6479320 B1, November 12, 2002. 44. Lee, C. C., Chen, Y.-C., and Matijasevic, G. “Au-In bonding below the eutectic temperature.” IEEE Trans. Component Packag. Manufact. Technol. 16:311–316, 1993. 45. Chen, Y.-C., and Lee, C. C. “Indium-copper multilayer composites for fluxless oxidation-free bonding.” Thin Solid Films 283:243–246, 1996. 46. Chen, Y.-C., So, W. W., and Lee, C. C. “A fluxless bonding technology using indium-silver multilayer composites.” IEEE Trans. Comp. Packag. Manufact. Technol. A 20:46–51, 1997. 47. Chuang, R. W., and Lee, C. C. “Silver-Indium joints produced at low temperature for high temperature devices.” IEEE Trans. Comp. Packag. Technol. 25:453–458, 2002. 48. Lee, C. C., and Choe, S. “Fluxless In-Sn bonding process at 140°C.” Mater. Sci. Eng. A 333:45–50, 2002.
205
206
Chapter Four 49. Sugiyama, S., Suzuki, T., Kawahata, K., Shimaoka, K., Takigawa, M., and Igarashi, I. “Micro-diaphragm pressure sensor.” IEEE Proceedings of IEDM’86, Los Angeles, CA, December 7–10, 1986, p. 184. 50. Ikeda, K., Kuwayama, H., Kobayashi, T., Watanabe, T., Nishikawa, T., Yoshida, T., and Harada, K. “Three-dimensional micromachining of silicon pressure sensor integrating resonant strain gauge on diaphragm.” Sensors & Actuators A 23:1007–1010, 1990. 51. Tabata, O., Shimaoka, K., and Sugiyama, S. “In situ observation and analysis of wet etching process for micro electro mechanical systems.” In Proceedings of IEEE MEMS’91, Nara, Japan, January 30–February 2, 1991, pp. 99–102. 52. Guckel, H., Sniegowski, J., Christenson, T. R., and Raissi, F. “The application of fine-grained, tensile polysilicon to mechanically resonant transducers.” Sensors & Actuators A A21–A23:346–351, 1990. 53. Lin, L., Howe, R. T., and Pisano, A. P. “Microelectromechanical filters for signal processing.” IEEE J. MEMS 7:286–294, 1998. 54. Partridge, A., Rice, A. E., Kenny, T. W., and Lutz, M. “New thin film epitaxial polysilicon encapsulation for pizeoresistivie accelerometers.” In IEEE Proceedings