NanoScience and Technology
NanoScience and Technology Series Editors: P. Avouris B. Bhushan K. von Klitzing H. Sakaki R. Wiesendanger The series NanoScience and Technology is focused on the fascinating nano-world, mesoscopic physics, analysis with atomic resolution, nano and quantum-effect devices, nanomechanics and atomic-scale processes. All the basic aspects and technology-oriented developments in this emerging discipline are covered by comprehensive and timely books. The series constitutes a survey of the relevant special topics, which are presented by leading experts in the field. These books will appeal to researchers, engineers, and advanced students.
Semiconductor Spintronics and Quantum Computation Editors: D.D. Awschalom, N. Samarth, D. Loss Nano-Optoelectonics Concepts, Physics and Devices Editor: M. Grundmann Noncontact Atomic Force Microscopy Editors: S. Morita, R. Wiesendanger, E. Meyer Nanoelectrodynamics Electrons and Electromagnetic Fields in Nanometer-Scale Structures Editor: H. Nejo Single Organic Nanoparticles Editors: H. Masuhara, H. Nakanishi, K. Sasaki Epitaxy of Nanostructures By V.A. Shchukin, N.N. Ledentsov and D. Bimberg Applied Scanning Probe Methods I Editors: B. Bhushan, H. Fuchs, S. Hosaka Nanostructures Theory and Modeling By C. Delerue and M. Lannoo Nanoscale Characterisation of Ferroelectric Materials Scanning Probe Microscopy Approach Editors: M. Alexe and A. Gruverman
Magnetic Microscopy of Nanostructures Editors: H. Hopster and H.P. Oepen Silicon Quantum Integrated Circuits Silicon-Germanium Heterostructure Devices: Basics and Realisations By E. Kasper, D.J. Paul The Physics of Nanotubes Fundamentals of Theory, Optics and Transport Devices Editors: S.V. Rotkin and S. Subramoney Single Molecule Chemistry and Physics An Introduction By C. Wang, C. Bai Atomic Force Microscopy, Scanning Nearfield Optical Microscopy and Nanoscratching Application to Rough and Natural Surfaces By G. Kaupp Applied Scanning Probe Methods II Scanning Probe Microscopy Techniques Editors: B. Bhushan, H. Fuchs Applied Scanning Probe Methods III Characterization Editors: B. Bhushan, H. Fuchs Applied Scanning Probe Methods IV Industrial Applications Editors: B. Bhushan, H. Fuchs
Bharat Bhushan Harald Fuchs (Eds.)
Applied Scanning Probe Methods II Scanning Probe Microscopy Techniques
With 263 Figures Including 7 Color Figures
123
Editors: Professor Bharat Bhushan Nanotribology Laboratory for Information Storage and MEMS/NEMS (NLIM) 650 Ackerman Road, Suite 255, The Ohio State University Columbus, OH 43202-1107, USA e-mail:
[email protected]
Professor Dr. Harald Fuchs Center for Nanotechnology (CeNTech) and Institute of Physics University of Münster, Gievenbecker Weg 11, 48149 Münster, Germany e-mail:
[email protected]
Series Editors: Professor Dr. Phaedon Avouris IBM Research Division, Nanometer Scale Science & Technology Thomas J. Watson Research Center, P.O. Box 218 Yorktown Heights, NY 10598, USA
Professor Bharat Bhushan Nanotribology Laboratory for Information Storage and MEMS/NEMS (NLIM) 650 Ackerman Road, Suite 255, The Ohio State University Columbus, OH 43202-1107, USA
Professor Dr., Dres. h. c. Klaus von Klitzing Max-Planck-Institut für Festkörperforschung, Heisenbergstrasse 1 70569 Stuttgart, Germany
Professor Hiroyuki Sakaki University of Tokyo, Institute of Industrial Science, 4-6-1 Komaba, Meguro-ku Tokyo 153-8505, Japan
Professor Dr. Roland Wiesendanger Institut für Angewandte Physik, Universität Hamburg, Jungiusstrasse 11 20355 Hamburg, Germany DOI 10.1007/b98404 ISSN 1434-4904 ISBN-10 3-540-26242-3 Springer Berlin Heidelberg New York ISBN-13 978-3-540-26242-8 Springer Berlin Heidelberg New York Library of Congress Control Number: 2003059049 This work is subject to copyright. All rights are reserved, whether the whole or part of the material is concerned, specifically the rights of translation, reprinting, reuse of illustrations, recitation, broadcasting, reproduction on microfilm or in any other way, and storage in data banks. Duplication of this publication or parts thereof is permitted only under the provisions of the German Copyright Law of September 9, 1965, in its current version, and permission for use must always be obtained from Springer. Violations are liable to prosecution under the German Copyright Law. Springer is a part of Springer Science+Business Media. springer.com © Springer-Verlag Berlin Heidelberg 2006 Printed in Germany The use of general descriptive names, registered names, trademarks, etc. in this publication does not imply, even in the absence of a specific statement, that such names are exempt from the relevant protective laws and regulations and therefore free for general use. Product liability: The publishers cannot guarantee the accuracy of any information about dosage and application contained in this book. In every individual case the user must check such information by consulting the relevant literature. Typesetting and production: LE-TEX Jelonek, Schmidt & Vöckler GbR, Leipzig Cover design : design & production, Heidelberg Printed on acid-free paper 2/3100/YL - 5 4 3 2 1 0
Foreword
The Nobel Prize of 1986 on Scanning Tunneling Microscopy signaled a new era in imaging. The scanning probes emerged as a new instrument for imaging with a precision sufficient to delineate single atoms. At first there were two – the Scanning Tunneling Microscope, or STM, and the Atomic Force Microscope, or AFM. The STM relies on electrons tunneling between tip and sample whereas the AFM depends on the force acting on the tip when it was placed near the sample. These were quickly followed by the Magnetic Force Microscope, MFM, and the Electrostatic Force Microscope, EFM. The MFM will image a single magnetic bit with features as small as 10 nm. With the EFM one can monitor the charge of a single electron. Prof. Paul Hansma at Santa Barbara opened the door even wider when he was able to image biological objects in aqueous environments. At this point the sluice gates were opened and a multitude of different instruments appeared. There are significant differences between the Scanning Probe Microscopes or SPM, and others such as the Scanning Electron Microscope or SEM. The probe microscopes do not require preparation of the sample and they operate in ambient atmosphere, whereas, the SEM must operate in a vacuum environment and the sample must be cross-sectioned to expose the proper surface. However, the SEM can record 3D image and movies, features that are not available with the scanning probes. The Near Field Optical Microscope or NSOM is also member of this family. At this time the instrument suffers from two limitations; 1) most of the optical energy is lost as it traverses the cut-off region of the tapered fiber and 2) the resolution is insufficient for many purposes. We are confident that NSOM’s with a reasonable optical throughput and a resolution of 10 nm will soon appear. The SNOM will then enter the mainstream of scanning probes.
VI
Foreword
In the Harmonic Force Microscope or HFM, the cantilever is driven at the resonant frequency with the amplitude adjusted so that the tip impacts the sample on each cycle. The forces between tip and sample generate multiple harmonics in the motion of the cantilever. The strength of these harmonics can be used to characterize the physical properties of the surface. It is interesting to note that this technology has spawned devices of a different kind. In one instance, the tip is functionalized in a way that allows the attachment of a single protein. Withdrawing the tip from a surface stretches the attached molecule and measures the elastic properties of single protein molecules. In another the surface tension on the surface of the cantilever is modified with a self-assembled monolayer of molecules such as thiols. The slight bending of the beam is easily detected with the components developed for use in the scanning probes. This system is used to detect the presence not only of the monomolecular layers but also of single molecules attached to the initial self-assembled monolayer. The extensive material in this field means that the variety of topics is larger than can be accommodated in four volumes. The Editors, Profs. Bhushan and Fuchs, must have great powers of persuasion for they have done a remarkable job in collecting this set of paper in a relatively short period of time. The collection will become a milestone in the field of scanning probes. c. f. quate Leland T. Edwards Professor (Research) of Engineering Stanford University Stanford, California Co-inventer of AFM in 1985
Preface
The rapidly increasing activities in nanoscience and nanotechnology supported by sizable national programs has led to a variety of efforts in the development and understanding of scanning probe techniques as well as their applications to industrial and medical environments. Beyond imaging, scanning probe techniques representing the eyes of nanotechnology allows us to investigate surfaces and interfaces close to surfaces at the nanometer scale and below, thus providing information about structure, mechanical, electronic, and magnetic properties. It became apparent during the collection phase of Vol. I in 2003 that many more activities exist which deserve presentation. Therefore, this three volume set was prepared in order to display the wide breadth of this field and also to provide an excellent compendium for recent developments in this area. The response of colleagues and research groups being asked to contribute has been very positive, such that we decided, together with the publisher, to rapidly move on in these areas. It became possible to collect excellent contributions displaying first hand information from leading laboratories worldwide. The present volumes II–IV cover three main areas: scanning probe microscopy (SPM) techniques (Vol. II); characterization (basic aspects, research, Vol. III); and industrial applications (Vol. IV). Volume II includes overviews on sensor technology based on SPM probes, high harmonic dynamic force microscopy, scanning ion conduction microscopy, spin polarized STM, dynamic force microscopy and spectroscopy, quantitative nanomechanical measurements in biology, scanning micro deformation microscopy, electrostatic force and force gradient microscopy and nearfield optical microscopy. This volume also includes a contribution on nearfield probe methods such as the scanning focus ion beam technique which is an extremely valuable tool for nanofabrication including scanning probes. Volume III includes the application of scanning probe methods for the characterization of different materials, mainly in the research stage, such as applications of SPM on living cells at high resolution, macromolecular dynamics, organic supramolecular structures under UHV conditions, STS on organic and inorganic low dimensional systems, and ferroelectric materials, morphological and tribological characterization of rough surfaces, AFM for contact and wear simulation, analysis of fullerene like nanoparticles and applications in the magnetic tape industry. The more relevant industrial applications are described in Vol. IV, which deals with scanning probe lithography for chemical, biological and engineering applications, nanofabrication with self-assembled monolayers by scanned probe lithography, fabrication of nanometer scale structures by local oxidation, template effects of
VIII
Preface
molecular assemblies, microfabricated cantilever arrays, nanothermomechanics and applications of heated atomic force microscope cantilevers. Certainly, the distinction between basic research fields of scanning probe techniques and the applications in industry are not sharp, as becomes apparent in the distribution of the individual articles in the different parts of these volumes. On the other hand, this clearly reflects an extremely active research field which strengthens the cooperation between nanotechnology and nanoscience. The success of the series is solely based on the efforts and the huge amount of work done by the authors. We gratefully acknowledge their excellent contributions in a timely manner which helps to inform scientists in research and industry about latest achievements in scanning probe methods. We also would like to thank Dr. Marion Hertel, Senior Editor Chemistry, and Mrs. Beate Siek of Springer Verlag for their continuous support, without which this volume could never make it efficiently to market. January, 2006
Prof. Bharat Bhushan, USA Prof. Harald Fuchs, Germany
Contents – Volume II
1
Higher Harmonics in Dynamic Atomic Force Microscopy Robert W. Stark, Martin Stark . . . . . . . . . . . . . . . . . . . .
1
1.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
1
1.2 1.2.1 1.2.2 1.2.3 1.2.4 1.2.5 1.2.6 1.2.7 1.2.8
Multimodal Model of the Microcantilever . . . Overview . . . . . . . . . . . . . . . . . . . . . Modal Analysis . . . . . . . . . . . . . . . . . Tip–Sample Interaction . . . . . . . . . . . . . State Space Formulation . . . . . . . . . . . . Dynamics: Linearized Tip–Sample Interaction Poles and Zeros . . . . . . . . . . . . . . . . . Dynamics: Nonlinear Interaction . . . . . . . . Optical Readout . . . . . . . . . . . . . . . . .
. . . . . . . . .
4 4 5 7 9 11 13 16 20
1.3
Higher Harmonic Imaging . . . . . . . . . . . . . . . . . . . . . .
23
1.4 1.4.1 1.4.2 1.4.3
Spectroscopy: Distinguishing Two Polymers Overview . . . . . . . . . . . . . . . . . . . . Experimental Details . . . . . . . . . . . . . Signal Analysis . . . . . . . . . . . . . . . .
. . . .
27 27 28 28
1.5
Outlook . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
33
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
33
2
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
. . . . . . . . .
. . . .
Atomic Force Acoustic Microscopy Ute Rabe . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
37
2.1 2.1.1 2.1.2 2.1.3
Introduction . . . . . . . . . . . . . . . . . . . . . Near-field Acoustic Microscopy . . . . . . . . . . Scanning Probe Techniques and Nanoindentation . Vibration Modes of AFM Cantilevers . . . . . . .
. . . .
. . . .
. . . .
38 39 40 41
2.2 2.2.1 2.2.2 2.2.3
Linear Contact-resonance Spectroscopy Using Flexural Modes Flexural Vibrations of Clamped-free Beams . . . . . . . . . . . The Point-mass Model . . . . . . . . . . . . . . . . . . . . . . Experiments with Clamped-free Beams . . . . . . . . . . . . .
. . . .
. . . .
42 44 47 48
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
X
Contents – Volume II
2.3
Contact Forces as Linear Springs and Dashpots . . . . . . . . . . .
51
2.4 2.4.1 2.4.2 2.4.3
Characteristic Equation of the Surface-coupled Beam Discussion of the Characteristic Equation . . . . . . . Influence of an Additional Mass . . . . . . . . . . . . Roots of the Characteristic Equation with Damping . .
. . . .
55 58 61 63
2.5
Forced Vibration . . . . . . . . . . . . . . . . . . . . . . . . . . . .
64
2.6
Imaging and Contrast Inversion . . . . . . . . . . . . . . . . . . .
70
2.7
Sensitivity of the Flexural Modes . . . . . . . . . . . . . . . . . . .
73
2.8 2.8.1
Quantitative Evaluation . . . . . . . . . . . . . . . . . . . . . . . . Experiments for Quantitative Evaluation . . . . . . . . . . . . . . .
76 78
2.9
Nonlinear Forces . . . . . . . . . . . . . . . . . . . . . . . . . . .
82
2.10
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
83
A A.1 A.2 A.3
Appendix . . . Definitions . . UAFM-mode . AFAM-mode .
. . . .
84 84 85 86
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
88
3
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
Scanning Ion Conductance Microscopy Tilman E. Schäffer, Boris Anczykowski, Harald Fuchs . . . . . . .
91
3.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
91
3.2 3.2.1 3.2.2 3.2.3
Fundamental Principles Basic Setup . . . . . . Nanopipettes . . . . . . Electrodes . . . . . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
92 92 95 96
3.3 3.3.1 3.3.2 3.3.3 3.3.4 3.3.5
Ion Currents Through Nanopipettes . . Background Theory . . . . . . . . . . . Simple Analytical Model . . . . . . . . Finite Element Modeling . . . . . . . . Experimental Current-Distance Curves Imaging with Ion Current Feedback . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
97 97 97 99 101 102
3.4 3.4.1 3.4.2
Advanced Techniques . . . . . . . . . . . . . . . . . . . . . . . . . Modulation Methods . . . . . . . . . . . . . . . . . . . . . . . . . Applications in Bioscience . . . . . . . . . . . . . . . . . . . . . .
103 104 106
3.5 3.5.1 3.5.2 3.5.3
Combination with Other Scanning Techniques Combination with Atomic Force Microscopy . Application in Material Science . . . . . . . . Combination with Shear Force Microscopy . .
107 108 108 111
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
Contents – Volume II
XI
3.5.4
Application in Bioscience . . . . . . . . . . . . . . . . . . . . . . .
114
3.6
Outlook . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
115
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
116
4
Spin-Polarized Scanning Tunneling Microscopy Wulf Wulfhekel, Uta Schlickum, Jürgen Kirschner . . . . . . . . . .
121
4.1 4.1.1 4.1.2 4.1.3
Introduction . . . . . . . . . . . . . . . . . . . The Resolution Problem in Magnetic Imaging Magnetism and Spin . . . . . . . . . . . . . . . The Tunneling Magnetoresistance Effect . . .
. . . .
. . . .
121 121 122 122
4.2 4.2.1 4.2.2 4.2.3
The Principle of Spin-polarized Scanning Tunneling Microscopy The Constant Current Mode . . . . . . . . . . . . . . . . . . . . The Spectroscopic Mode . . . . . . . . . . . . . . . . . . . . . . Differential Magnetic Imaging Mode . . . . . . . . . . . . . . .
. . . .
124 125 125 126
4.3
Experimental Set-up . . . . . . . . . . . . . . . . . . . . . . . . . .
127
4.4 4.4.1 4.4.2
Ferromagnetic Domains and Domain Walls . . . . . . . . . . . . . Ultra-sharp Domain Walls in Co(0001) . . . . . . . . . . . . . . . Asymmetric Néel Caps in Fe(001) . . . . . . . . . . . . . . . . . .
128 129 131
4.5 4.5.1 4.5.2
Antiferromagnets in Contact with Ferromagnets . . . . . . . . . . Mn on Fe(001) and Topologically Induced Frustrations . . . . . . The Layered Antiferromagnet Cr on Fe(001) . . . . . . . . . . . .
133 133 136
4.6 4.6.1 4.6.2
Bulk Versus Surface: Which Electronic States Cause the Spin Contrast? . . . . . . . . . Voltage Dependence of the TMR Effect in Co(0001) . . . . . . . . Voltage Dependence of the TMR Effect in Cr/Fe(001) . . . . . . .
137 137 139
4.7
Conclusion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
140
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
140
5
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
Dynamic Force Microscopy and Spectroscopy Ferry Kienberger, Hermann Gruber, Peter Hinterdorfer . . . . . .
143
5.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
144
5.2
Scanning Probe Microscopy . . . . . . . . . . . . . . . . . . . . .
145
5.3
Dynamic Force Microscopy Imaging . . . . . . . . . . . . . . . . .
146
5.4 5.4.1 5.4.2 5.4.3
Force Spectroscopy Principles . . . . . Theory . . . . . . . Applications . . . .
149 149 151 153
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
XII
Contents – Volume II
5.5
Combined Imaging and Spectroscopy . . . . . . . . . . . . . . . .
158
5.6
Concluding Remarks . . . . . . . . . . . . . . . . . . . . . . . . .
161
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
161
6
Sensor Technology for Scanning Probe Microscopy and New Applications Egbert Oesterschulze, Leon Abelmann, Arnout van den Bos, Rainer Kassing, Nicole Lawrence, Gunther Wittstock, Christiane Ziegler . . . . . . . . . . . . . . . . . . . . . . . . . . . 165
6.1
Introductory Remarks . . . . . . . . . . . . . . . . . . . . . . . . .
165
6.2 6.2.1
Material Aspects of Probe Fabrication . . . . . . . . . . . . . . . . Mechanical Properties of Cantilever Probes . . . . . . . . . . . . .
166 167
6.3 6.3.1 6.3.2
Scanning Near-Field Optical Microscopy . . . . . . . . . . . . . . Principle of Near-Field Optics . . . . . . . . . . . . . . . . . . . . Probes for Scanning Near-Field Optical Microscopy (SNOM) . . .
174 174 175
6.4 6.4.1
Probes for Ultrafast Scanning Probe Microscopy . . . . . . . . . . Improved Sampling Technique . . . . . . . . . . . . . . . . . . . .
179 181
6.5 6.5.1 6.5.2
Functionalized Tips . . . . . . . . . . . . . . . . . . . . . . . . . . Tip Modification . . . . . . . . . . . . . . . . . . . . . . . . . . . . Applications . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
182 182 183
6.6 6.6.1 6.6.2
Scanning Electrochemical Microscopy . . . . . . . . . . . . . . . . Principles . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Applications . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
186 186 189
6.7 6.7.1 6.7.2 6.7.3 6.7.4
Tips for Magnetic Force Microscopy . Ideal Tip Shape . . . . . . . . . . . . Hand-Made Tips . . . . . . . . . . . . Coating AFM Tips . . . . . . . . . . Tip Planes: The CantiClever Concept
. . . . .
192 192 193 194 195
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
197
7
7.1 7.1.1 7.1.2 7.1.3 7.1.4
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
Quantitative Nanomechanical Measurements in Biology Małgorzata Lekka, Andrzej J. Kulik . . . . . . . . . . . . . . . . . Stiffness of Biological Samples . . . . . . . Cell Structure . . . . . . . . . . . . . . . . Determination of Young’s Modulus . . . . Brief Overview of the Application of AFM to Studies of Living Cells . . . . . . . . . . Summary . . . . . . . . . . . . . . . . . . .
205
. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
205 205 208
. . . . . . . . . . . . . . . . . . . . . . . . . .
217 222
Contents – Volume II
7.2 7.2.1 7.2.2 7.2.3
XIII
. . . .
224 225 229 236
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
237
8
Friction Force Microscopy . . . . . . . . Friction and Chemical Force Microscopy Applications of FFM/CFM . . . . . . . . Summary . . . . . . . . . . . . . . . . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
Scanning Microdeformation Microscopy: Subsurface Imaging and Measurement of Elastic Constants at Mesoscopic Scale Pascal Vairac, Bernard Cretin . . . . . . . . . . . . . . . . . . . .
241
8.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
241
8.2
Review and Physical Background of Near-Field Acoustic Microscopes . . . . . . . . . . . . . . . . . . . . . . Review of Near-Field Microscopes . . . . . . . . . . . . . . . Physical Basis for Near-Field Acoustics and the Scale Effect Mechanical Approach . . . . . . . . . . . . . . . . . . . . . . Models of Subsurface Sensing Using Acoustic Waves and Surface Bending . . . . . . . . . . . . . . . . . . . . . .
. . . .
242 242 244 247
. . .
252
8.3.1 8.3.2 8.3.3
Imaging and Measurement with Scanning Microdeformation Microscopy . . . . . . . . . . . . . . . . . . . . . . . . . . . Configuration . . . . . . . . . . . . . . . . . . . . . . . . . . Application to Subsurface Imaging . . . . . . . . . . . . . . . Characterization of Local Mechanical Constants . . . . . . .
. . . .
. . . .
. . . .
254 254 256 259
8.4 8.4.1 8.4.2 8.4.3
Specific Application . . . Thin Film Measurements Shape Memory Alloy . . Viscosimetry . . . . . . .
. . . .
. . . .
. . . .
260 260 264 267
8.5
Ultimate Metrology: Measurements at the Mechanical Noise Level
274
8.6
Conclusion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
278
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
279
8.2.1 8.2.2 8.2.3 8.2.4 8.3
9
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
Electrostatic Force and Force Gradient Microscopy: Principles, Points of Interest and Application to Characterisation of Semiconductor Materials and Devices Paul Girard, Alexander Nikolaevitch Titkov . . . . . . . . . . . . .
283
9.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
285
9.2 9.2.1 9.2.2
Principles . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Basic Relations . . . . . . . . . . . . . . . . . . . . . . . . . . . . Principles of Surface-voltage Measurements . . . . . . . . . . . .
285 286 287
XIV
9.2.3
Contents – Volume II
9.2.4
Detection of Strong Local Electrical Effect via the “Topographic” Data . . . . . . . . . . . . . . . . . . . . . . Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
294 296
9.3 9.3.1 9.3.2 9.3.3 9.3.4 9.3.5
Observation and Interpretation DC Observations . . . . . . . Ω Observations . . . . . . . . 2Ω Observations . . . . . . . Surface Voltage Observations . Guidelines for Interpretation .
. . . . . .
297 299 300 300 302 302
9.4 9.4.1 9.4.2 9.4.3
Future Opportunities . . . . . . . . . . . . . . . Interest in the KFGM Method . . . . . . . . . . Spatially Resolved Observations . . . . . . . . . Another Way to Estimate the Maximum Possible Spatial Resolution . . . . . . . . . . . . . . . . .
. . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
304 304 309
. . . . . . . . . .
311
9.5 9.5.1 9.5.2
Some Applications . . . . . . . . . . . . . . . . . . . . . . . . . . Applications Under Ambient Conditions . . . . . . . . . . . . . . Vacuum or UHV Applications . . . . . . . . . . . . . . . . . . . .
313 314 316
9.6
Conclusion . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
316
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
318
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
10
Polarization-Modulation Techniques in Near-Field Optical Microscopy for Imaging of Polarization Anisotropy in Photonic Nanostructures Pietro Giuseppe Gucciardi, Ruggero Micheletto, Yoichi Kawakami, Maria Allegrini . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 321
10.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
321
10.2 10.2.1
Polarimetric Imaging . . . . . . . . . . . . . . . . . . . . . . . . . The Jones Formalism . . . . . . . . . . . . . . . . . . . . . . . . .
322 325
10.3
Electromagnetic Field Diffracted by a SNOM Aperture . . . . . .
327
10.4 10.4.1 10.4.2 10.4.3
Experimental Implementations . . . . . . . . . . . . Static Polarization SNOM . . . . . . . . . . . . . . Polarization-Modulation SNOM: Illumination Mode Polarization-Modulation SNOM: Collection Mode .
. . . .
. . . .
. . . .
. . . .
. . . .
333 333 337 342
10.5 10.5.1 10.5.2 10.5.3 10.5.4 10.5.5
Applications of SNOM Polarimetry . . . . . . . . . . . . . Polarization Responses of Photonic Waveguides . . . . . . Measuring Stress-Induced Birefringence . . . . . . . . . . . Polarization Anisotropy in Mesoscale-Structured Materials Polarization Anisotropy in Polymers . . . . . . . . . . . . . Polarization Anisotropy in Photoluminescence Emission . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
344 345 348 349 351 354
10.6
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
357
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
357
. . . .
. . . .
. . . .
Contents – Volume II
11
XV
Focused Ion Beam as a Scanning Probe: Methods and Applications Vittoria Raffa, Piero Castrataro, Arianna Menciassi, Paolo Dario .
361
11.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
361
11.2 11.2.1 11.2.2 11.2.3 11.2.4
Description of the System . . . . . System Overview . . . . . . . . . Liquid Metal Ion Source (LMIS) . Ion Optics . . . . . . . . . . . . . Dual Beam Systems . . . . . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
362 362 363 364 365
11.3 11.3.1 11.3.2 11.3.3 11.3.4 11.3.5
FIB Processes . . . . . . Imaging . . . . . . . . . Milling . . . . . . . . . . Gas-Assisted Etching . . Gas-Assisted Deposition Ion Beam Lithography .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
367 367 372 376 377 379
11.4 11.4.1 11.4.2 11.4.3
Main Applications . . . . . . . . . . FIB as an Analytical Technique . . FIB in the Semiconductor Industry . Micromachining . . . . . . . . . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
380 381 389 401
11.5
Future Directions . . . . . . . . . . . . . . . . . . . . . . . . . . .
408
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
409
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
Subject Index . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 413
Contents – Volume III
12
Atomic Force Microscopy in Nanomedicine Dessy Nikova, Tobias Lange, Hans Oberleithner, Hermann Schillers, Andreas Ebner, Peter Hinterdorfer . . . . . . .
1
12.1
AFM in Biological Sciences . . . . . . . . . . . . . . . . . . . . .
1
12.2 12.2.1 12.2.2 12.2.3 12.2.4 12.2.5
Plasma Membrane Preparation for AFM Imaging . . . . . Introduction . . . . . . . . . . . . . . . . . . . . . . . . . Plasma Membrane Preparation . . . . . . . . . . . . . . . Atomic Force Microscopy . . . . . . . . . . . . . . . . . Molecular Volume Measurements of Membrane Proteins . AFM Imaging . . . . . . . . . . . . . . . . . . . . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
4 4 5 7 7 7
12.3 12.3.1 12.3.2 12.3.3
AFM Imaging of CFTR in Oocyte Membranes Introduction . . . . . . . . . . . . . . . . . . . Does the CFTR Form Functional Assemblies? Two CFTRs are Better Than One . . . . . . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
10 11 11 13
12.4 12.4.1 12.4.2 12.4.3 12.4.4
Single Antibody–CFTR Recognition Imaging . Introduction . . . . . . . . . . . . . . . . . . . Tethering of Antibodies to AFM Tips . . . . . AFM Imaging and Recognition . . . . . . . . . A Single Antibody Sees a Single CFTR . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
16 16 17 17 17
12.5 12.5.1 12.5.2 12.5.3
Single Cell Elasticity: Probing for Diseases Introduction . . . . . . . . . . . . . . . . . Force–Mapping AFM . . . . . . . . . . . . Can One Protein Change Cell Elasticity? .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
19 19 20 21
12.6
Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
24
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
24
. . . .
. . . .
XVIII
13
Contents – Volume III
Scanning Probe Microscopy: From Living Cells to the Subatomic Range Ille C. Gebeshuber, Manfred Drack, Friedrich Aumayr, Hannspeter Winter, Friedrich Franek . . . . . . . . . . . . . . . . .
27
13.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
27
13.2 13.2.1 13.2.2
Cells In Vivo as Exemplified by Diatoms . . . . . . . . . . . . . . Introduction to Diatoms . . . . . . . . . . . . . . . . . . . . . . . . SPM of Diatoms . . . . . . . . . . . . . . . . . . . . . . . . . . . .
28 28 30
13.3
Interaction of Large Organic Molecules . . . . . . . . . . . . . . .
33
13.4 13.4.1 13.4.2
Nanodefects on Atomically Flat Surfaces . . . . . . . . . . . . . . Ion Bombardment of Highly Oriented Pyrolytic Graphite (HOPG) Bombardment of Single Crystal Insulators with Multicharged Ions
37 38 42
13.5 13.5.1 13.5.2
Subatomic Features . . . . . . . . . . . . . . . . . . . . . . . . . . Atom Orbitals . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Single Electron Spin Detection with AFM and STM . . . . . . . .
45 45 47
13.6
Conclusions and Outlook . . . . . . . . . . . . . . . . . . . . . . .
50
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
51
14
Surface Characterization and Adhesion and Friction Properties of Hydrophobic Leaf Surfaces and Nanopatterned Polymers for Superhydrophobic Surfaces Zachary Burton, Bharat Bhushan . . . . . . . . . . . . . . . . . .
55
14.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
55
14.2 14.2.1 14.2.2 14.2.3 14.2.4
Experimental Details . . . . . . . . . . . Instrumentation . . . . . . . . . . . . . . Samples . . . . . . . . . . . . . . . . . . Roughness Factor . . . . . . . . . . . . . Test Matrix for Nanopatterned Polymers .
. . . . .
58 58 59 61 62
14.3 14.3.1 14.3.2
Results and Discussion . . . . . . . . . . . . . . . . . . . . . . . . Hydrophobic Leaf Surfaces . . . . . . . . . . . . . . . . . . . . . . Nanopatterned Polymers . . . . . . . . . . . . . . . . . . . . . . .
63 64 74
14.4
Summary . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
79
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
81
15
15.1
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
Probing Macromolecular Dynamics and the Influence of Finite Size Effects Scott Sills, René M. Overney . . . . . . . . . . . . . . . . . . . . .
83
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
84
Contents – Volume III
XIX
15.2
The Glass Transition and Molecular Mobility . . . . . . . . . . . .
85
15.3 15.3.1 15.3.2 15.3.3 15.3.4 15.3.5 15.3.6
Macromolecular Probing Techniques . . . . . . . . . . . . . Static Contacts . . . . . . . . . . . . . . . . . . . . . . . . . . Modulated Contacts . . . . . . . . . . . . . . . . . . . . . . . Calibration of Lateral Forces in Scanning Probe Microscopy . Shear Modulation Force Microscopy (SM-FM) . . . . . . . . Friction Force Microscopy (FFM) . . . . . . . . . . . . . . . Tribological Models for FFM . . . . . . . . . . . . . . . . . .
. . . . . . .
90 90 92 93 97 98 99
15.4 15.4.1 15.4.2 15.4.3
Internal Friction and Dynamics near the Glass Transition . . . . . Molecular Relaxations . . . . . . . . . . . . . . . . . . . . . . . . Structural Heterogeneity and Relaxation near the Glass Transition Cooperative Molecular Motion During the Glass Transition . . . .
103 103 105 107
15.5 15.5.1 15.5.2 15.5.3 15.5.4
Constraints and Structural Modifications near Interfaces Interfacial Plasticization . . . . . . . . . . . . . . . . . . Dewetting Kinetics . . . . . . . . . . . . . . . . . . . . Disentanglement Barriers . . . . . . . . . . . . . . . . . Interfacial Glass Transition Profiles . . . . . . . . . . .
. . . . .
. . . . .
109 109 110 111 113
15.6 15.6.1 15.6.2 15.6.3
Mechanical Operations in Nanoscopic Polymer Systems Indentation Contact Mechanics . . . . . . . . . . . . . . Rim Formation During Indentation . . . . . . . . . . . . Strain Shielding and Confined Plasticity in Nanoscopic Polymer Systems . . . . . . . . . . . . .
. . . . . . . . . . . . . . . . . .
115 116 120
. . . . . .
122
Closing Remarks . . . . . . . . . . . . . . . . . . . . . . . . . . .
126
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
127
15.7
16
. . . . .
. . . . .
. . . . . . .
. . . . .
. . . . . . .
. . . . .
Investigation of Organic Supramolecules by Scanning Probe Microscopy in Ultra-High Vacuum Laurent Nony, Enrico Gnecco, Ernst Meyer . . . . . . . . . . . . .
131
16.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
131
16.2 16.2.1 16.2.2 16.2.3
Methods . . . . . . . . . . . . . . . . . . . Organic Molecular Beam Epitaxy (OMBE) Scanning Tunneling Microscopy (STM) . . Atomic Force Microscopy (AFM) . . . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
132 132 134 137
16.3 16.3.1 16.3.2 16.3.3 16.3.4 16.3.5 16.3.6 16.3.7
Molecules . . . . . . . . . . Fullerenes . . . . . . . . . . Porphyrins . . . . . . . . . . Phthalocyanines . . . . . . . Perylene Derivatives . . . . . Lander Molecules . . . . . . PVBA Molecules . . . . . . Decacyclene and Derivatives
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
142 142 142 142 144 144 144 144
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
XX
Contents – Volume III
16.4 16.4.1 16.4.2
Molecules on Metals . . . . . . . . . . . . . . . . . . . . . . . . . STM Investigations . . . . . . . . . . . . . . . . . . . . . . . . . . Non-Contact AFM Investigations . . . . . . . . . . . . . . . . . .
145 145 157
16.5 16.5.1 16.5.2
Molecules on Semiconductor Surfaces . . . . . . . . . . . . . . . . STM Investigations . . . . . . . . . . . . . . . . . . . . . . . . . . Non-Contact AFM Investigations . . . . . . . . . . . . . . . . . .
162 162 165
16.6 16.6.1 16.6.2
Molecules on Insulating Surfaces . . . . . . . . . . . . . . . . . . . STM Investigations . . . . . . . . . . . . . . . . . . . . . . . . . . Non-contact AFM Investigations . . . . . . . . . . . . . . . . . . .
167 168 169
16.7 16.7.1 16.7.2
Manipulation of Single Molecules . . . . . . . . . . . . . . . . . . STM Investigations . . . . . . . . . . . . . . . . . . . . . . . . . . Non-contact AFM Investigations . . . . . . . . . . . . . . . . . . .
171 171 175
16.8
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
175
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
176
17
One- and Two-Dimensional Systems: Scanning Tunneling Microscopy and Spectroscopy of Organic and Inorganic Structures Luca Gavioli, Massimo Sancrotti . . . . . . . . . . . . . . . . . . .
183
17.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
183
17.2
Basic Principles of STM and STS . . . . . . . . . . . . . . . . . .
185
17.3 17.3.1 17.3.2
Inorganic Overlayers . . . . . . . . . . . . . . . . . . . . . . . . . 1D Structures . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 2D Structures . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
188 188 196
17.4 17.4.1 17.4.2
Molecular Overlayers . . . . . . . . . . . . . . . . . . . . . . . . . 1D Structures . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 2D Overlayers . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
201 202 208
17.5
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
212
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
212
18
Scanning Probe Microscopy Applied to Ferroelectric Materials Oleg Tikhomirov, Massimiliano Labardi, Maria Allegrini . . . . . .
217
18.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
217
18.2
Development of Scanning Probe Techniques for Ferroelectrics . .
217
18.3 18.3.1 18.3.2 18.3.3
Scanning Force Microscopy Non-Contact Mode . . . . . Contact Mode . . . . . . . . Voltage-Modulated SFM . .
220 220 221 222
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
Contents – Volume III
XXI
18.3.4 18.3.5 18.3.6 18.3.7 18.3.8
Resonance Modes of EFM Lateral Force . . . . . . . . Frontal Force . . . . . . . . Second Harmonic . . . . . Tapping Mode . . . . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
224 228 232 233 234
18.4 18.4.1 18.4.2 18.4.3 18.4.4 18.4.5
Scanning Optical Microscopy . . . Pure Optical Microscopy . . . . . . Scanning Electrooptic Microscopy . Near-Field Electrooptic Microscopy Micro-Spectroscopic Techniques . . Second Harmonic Microscopy . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
235 235 237 242 244 245
18.5 18.5.1 18.5.2 18.5.3 18.5.4 18.5.5 18.5.6 18.5.7
Applications to Ferroelectrics . . . . . . Imaging of Domains and Domain Walls Writing Patterns . . . . . . . . . . . . . Phase Transitions . . . . . . . . . . . . Morphotropic Phase Boundary . . . . . Relaxors . . . . . . . . . . . . . . . . . Thin Films . . . . . . . . . . . . . . . . Artificial Nanostructures . . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
. . . . . . . .
247 247 248 249 250 251 251 252
18.6
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
253
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
254
19
. . . . .
. . . . .
. . . . .
. . . . .
Morphological and Tribological Characterization of Rough Surfaces by Atomic Force Microscopy Renato Buzio, Ugo Valbusa . . . . . . . . . . . . . . . . . . . . . .
261
19.1.1 19.1.2 19.1.3
Characterization of Surface Roughness by Atomic Force Microscopy . . . . . . . . . . . . . . . . . . . . . Statistical Methods for Stationary Random Surfaces . . . . . . . . Statistical Methods for Fractal Surfaces . . . . . . . . . . . . . . . Estimation of Morphological Parameters from AFM Topographies
263 264 266 270
19.2 19.2.1 19.2.2 19.2.3
Modeling Contact Mechanics for Rough Surfaces . . Early Phenomenological Contact Theories . . . . . Contact Mechanics Theories for Fractal Roughness . On the Molecular Origins of Amontons’ Law . . . .
. . . .
272 273 277 284
19.3 19.3.1
. . . .
286
19.3.2 19.3.3
Investigations of Multi-Asperity Contacts by AFM . . . . . AFM Characterization of Surface Roughness for Tribological Purposes . . . . . . . . . . . . . . . . . . . Contact Mechanics Investigations at the Nanometer Scale . Contact Mechanics Investigations on the Micrometer Scale
. . . . . . . . . . . .
286 288 291
19.4
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
293
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
294
19.1
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
XXII
20
Contents – Volume III
AFM Applications for Contact and Wear Simulation Nikolai K. Myshkin, Mark I. Petrokovets, Alexander V. Kovalev . .
299
20.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
299
20.2
Scale Factor in Tribology . . . . . . . . . . . . . . . . . . . . . . .
299
20.3 20.3.1 20.3.2 20.3.3 20.3.4 20.3.5
AFM as a Tool of Contact Simulation . . . Contact of Rough Surfaces . . . . . . . . . Rough Contact with Adhesion . . . . . . . Multilevel Contact Models . . . . . . . . . Simulation of Contact Using AFM Images Nanomechanical Probing of Soft Layers . .
. . . . . .
300 300 303 307 309 312
20.4 20.4.1 20.4.2
AFM in Wear Simulation . . . . . . . . . . . . . . . . . . . . . . . Nanoscratching and Nanowear with AFM Tip . . . . . . . . . . . . Wear Simulation in AFM Contact Mode . . . . . . . . . . . . . . .
316 317 320
20.5
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
323
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
324
21
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
. . . . . .
AFM Applications for Analysis of Fullerene-Like Nanoparticles Lev Rapoport, Armen Verdyan . . . . . . . . . . . . . . . . . . . .
327
21.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
327
21.2 21.2.1 21.2.2
Instrumentation . . . . . . . . . . . . . . . . . . . . . . . . . . . . Friction Experiment . . . . . . . . . . . . . . . . . . . . . . . . . . AFM Experiment . . . . . . . . . . . . . . . . . . . . . . . . . . .
328 328 329
21.3
Characterization of Fullerene-Like Solid Lubricant Nanoparticles .
330
21.4
Friction of Solid Lubricant Films . . . . . . . . . . . . . . . . . . .
331
21.5
Friction and Wear of the Surfaces Lubricated with Oil + IF Nanoparticles . . . . . . . . . . . . . . . . . . . . . .
333
21.6
Friction of IF Nanoparticles Under Severe Contact Conditions . .
336
21.7
Mechanisms of Friction of the IF Nanoparticles . . . . . . . . . .
339
21.8
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
341
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
341
22
Scanning Probe Methods in the Magnetic Tape Industry James K. Knudsen . . . . . . . . . . . . . . . . . . . . . . . . . . .
343
22.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
343
22.2
Atomic Force Microscopy . . . . . . . . . . . . . . . . . . . . . .
345
Contents – Volume III
XXIII
22.2.1 22.2.2 22.2.3
Topographic Characterization of the Magnetic Tape . . . . . . . . Topographic Characterization of Heads . . . . . . . . . . . . . . . Tape Roughness Analysis . . . . . . . . . . . . . . . . . . . . . . .
345 349 351
22.3 22.3.1 22.3.2 22.3.3
Magnetic Force Microscopy . . . . . . . . . . . . Methodology . . . . . . . . . . . . . . . . . . . . . Characterization of the Magnetic Tape with MFM Characterization of Heads with MFM . . . . . . .
. . . .
358 358 359 364
22.4
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
367
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
367
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
Subject Index . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 371
Contents – Volume IV
23
Scanning Probe Lithography for Chemical, Biological and Engineering Applications Joseph M. Kinsella, Albena Ivanisevic . . . . . . . . . . . . . . . .
1
23.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
2
23.2
Modeling of the DPN Process . . . . . . . . . . . . . . . . . . . .
4
23.3 23.3.1 23.3.2 23.3.3 23.3.4
Patterning of Biological and Biologically Active Molecules . DNA Patterning . . . . . . . . . . . . . . . . . . . . . . . . . Protein Patterning . . . . . . . . . . . . . . . . . . . . . . . . Peptide Patterning . . . . . . . . . . . . . . . . . . . . . . . . Patterning of Templates for Biological Bottom-Up Assembly
. . . . .
. . . . .
. . . . .
7 8 10 13 15
23.4 23.4.1 23.4.2 23.4.3 23.4.4 23.4.5 23.4.6 23.4.7 23.4.8 23.4.9 23.4.10 23.4.11
Chemical Patterning . . . . . . . . . . . . Thiols . . . . . . . . . . . . . . . . . . . ω-Substituted Thiols . . . . . . . . . . . Silanes and Silazanes . . . . . . . . . . . Deposition of Solid Organic Inks . . . . . Polymers . . . . . . . . . . . . . . . . . . Polyelectrolytes . . . . . . . . . . . . . . Dendrimers . . . . . . . . . . . . . . . . Deposition of Supramolecular Materials . Deposition of Metals . . . . . . . . . . . Deposition of Solid-State Materials . . . Deposition of Magnetic Materials . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
17 17 18 19 20 21 23 23 24 25 26 27
23.5
Engineering Applications of DPN . . . . . . . . . . . . . . . . . .
28
23.6
Future Challenges and Applications . . . . . . . . . . . . . . . . .
30
23.7
Conclusions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
31
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
31
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
. . . . . . . . . . . .
XXVI
24
Contents – Volume IV
Nanotribological Characterization of Human Hair and Skin Using Atomic Force Microscopy (AFM) Bharat Bhushan, Carmen LaTorre . . . . . . . . . . . . . . . . . .
35
24.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
35
24.2 24.2.1 24.2.2
Human Hair, Skin, and Hair Care Products . . . . . . . . . . . . . Human Hair and Skin . . . . . . . . . . . . . . . . . . . . . . . . . Hair Care: Cleaning and Conditioning Treatments, and Damaging Processes . . . . . . . . . . . . . . . . . . . . . . .
39 39
24.3 24.3.1 24.3.2
Experimental Techniques . . . . . . . . . . . . . . . . . . . . . . . Experimental Procedure . . . . . . . . . . . . . . . . . . . . . . . . Hair and Skin Samples . . . . . . . . . . . . . . . . . . . . . . . .
51 53 57
24.4 24.4.1
. .
59
. .
59
. .
70
. .
78
24.4.5
Results and Discussion . . . . . . . . . . . . . . . . . . . . . . Surface Roughness, Friction, and Adhesion for Various Ethnicities of Hair . . . . . . . . . . . . . . . . . . Surface Roughness, Friction, and Adhesion for Virgin and Chemically Damaged Caucasian Hair (with and without Commercial Conditioner Treatment) . . . . . Surface Roughness, Friction, and Adhesion for Hair Treated with Various Combinations of Conditioner Ingredients Investigation of Directionality Dependence and Scale Effects on Friction and Adhesion of Hair . . . . . . . . . . . . . . . . . Surface Roughness and Friction of Skin . . . . . . . . . . . . .
. . . .
85 98
24.5
Closure . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
98
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
102
Appendix . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
103
24.4.2
24.4.3 24.4.4
25
46
Nanofabrication with Self-Assembled Monolayers by Scanning Probe Lithography Jayne C. Garno, James D. Batteas . . . . . . . . . . . . . . . . . .
105
25.1 25.1.1 25.1.2 25.1.3 25.1.4
SPM-Based Methods of Lithography . . Bias-Induced Nanofabrication . . . . . . Force-Induced Nanofabrication of SAMs Dip-Pen Nanolithography (DPN) . . . . . Automated Scanning Probe Lithography .
. . . . .
105 107 108 110 111
25.2 25.2.1 25.2.2 25.2.3
Patterning with Self-Assembled Monolayers . . . . . . . . . . . . Structure of SAMs . . . . . . . . . . . . . . . . . . . . . . . . . . . Examples of SAM Nanopatterns Generated by Force-Induced SPL Nanofabrication of SAMs by DPN and Bias-Induced SPL . . . . .
112 112 114 118
25.3
Directed Fabrication of Polymeric Structures . . . . . . . . . . . .
120
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
Contents – Volume IV
XXVII
25.4
Fabrication of Metallic Structures . . . . . . . . . . . . . . . . . .
122
25.5 25.5.1 25.5.2 25.5.3
Nanoscale Patterning of Proteins . . . . . . . . . . . . Protein Arrays Generated by DPN . . . . . . . . . . . Applying Bias-Induced SPL for Protein Nanopatterns Protein Immobilization on SAMs Generated by Force-Induced SPL . . . . . . . . . . .
. . . . . . . . . . . . . . . . . . . . .
126 127 128
. . . . . . .
129
Conclusions and Outlook . . . . . . . . . . . . . . . . . . . . . . .
130
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
131
25.6
26
Fabrication of Nanometer-Scale Structures by Local Oxidation Nanolithography Marta Tello, Fernando García, Ricardo García . . . . . . . . . . .
137
26.1
Introduction to AFM Nanolithographies . . . . . . . . . . . . . . .
137
26.2
Basic Local Oxidation Aspects . . . . . . . . . . . . . . . . . . . .
138
26.3
Mechanism and Kinetics . . . . . . . . . . . . . . . . . . . . . . .
141
26.4
Feature Size . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
143
26.5
Applications I: Patterning, Data Storage and Template Growth . .
146
26.6
Applications II: Nanoelectronic Devices . . . . . . . . . . . . . . .
151
26.7
Parallel Oxidation . . . . . . . . . . . . . . . . . . . . . . . . . . .
154
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
155
27
Template Effects of Molecular Assemblies Studied by Scanning Tunneling Microscopy (STM) Chen Wang, Chunli Bai . . . . . . . . . . . . . . . . . . . . . . . .
159
27.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
159
27.2
27.2.2 27.2.3 27.2.4
Single Guest Molecule Immobilization with Assembled Molecular Networks . . . . . Hydrogen Bonded Supramolecular Networks and Single Molecule Inclusions . . . . . . . . Van der Waals Interaction Stabilized Networks Metal-Organic Coordination Networks . . . . Covalently Bonded Molecular Grids . . . . . .
. . . . . . . . . . .
160
. . . .
. . . .
160 163 165 166
27.3 27.3.1 27.3.2
Intralayer Heterogeneous Molecular Arrays . . . . . . . . . . . . . Hydrogen Bond Stabilized Heterogeneous Lamellae . . . . . . . . Van der Waals Interaction Stabilized Intralayer Arrays . . . . . . .
166 167 168
27.4 27.4.1
Interlayer Effect on Molecular Adsorption and Assemblies . . . . Site Selective Adsorption . . . . . . . . . . . . . . . . . . . . . . .
171 172
27.2.1
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
. . . .
XXVIII
Contents – Volume IV
27.4.2 27.4.3
Molecular Arrays . . . . . . . . . . . . . . . . . . . . . . . . . . . Directional Assembly of Nanoparticle Arrays . . . . . . . . . . . .
176 177
27.5
Future Perspectives . . . . . . . . . . . . . . . . . . . . . . . . . .
179
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
179
28
Microfabricated Cantilever Array Sensors for (Bio-)Chemical Detection Hans Peter Lang, Martin Hegner, Christoph Gerber . . . . . . . .
183
28.1 28.1.1 28.1.2 28.1.3 28.1.4
Introduction . . . . . . . . . Sensors . . . . . . . . . . . . Cantilevers . . . . . . . . . . Cantilever Operating Modes Cantilever Arrays . . . . . .
. . . . .
183 183 184 186 192
28.2 28.2.1 28.2.2
Experimental Setup . . . . . . . . . . . . . . . . . . . . . . . . . . Measurement Chamber . . . . . . . . . . . . . . . . . . . . . . . . Cantilever Functionalization . . . . . . . . . . . . . . . . . . . . .
196 196 198
28.3 28.3.1 28.3.2
Measurements . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Artificial Nose for Detection of Perfume Essences . . . . . . . . . Label-Free DNA Hybridization Detection . . . . . . . . . . . . . .
203 204 206
28.4
Applications and Outlook . . . . . . . . . . . . . . . . . . . . . . .
209
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
210
29
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
Nano-Thermomechanics: Fundamentals and Application in Data Storage Devices B. Gotsmann, U. Dürig . . . . . . . . . . . . . . . . . . . . . . . .
215
29.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
215
29.2 29.2.1 29.2.2 29.2.3 29.2.4
Heat Transfer Mechanisms . . . . . . . . . . . . . . Heat Generation in Microcantilevers . . . . . . . . . Heat Transfer Through Air and Silicon . . . . . . . Heat Transfer Through Radiation . . . . . . . . . . . Heat Transfer Through a Tip-Surface Point Contact
. . . . .
215 216 217 222 224
29.3
Momentum Transfer Through Air . . . . . . . . . . . . . . . . . .
227
29.4 29.4.1 29.4.2 29.4.3 29.4.4 29.4.5 29.4.6 29.4.7
Thermomechanical Nanoindentation of Polymers . . . General Considerations . . . . . . . . . . . . . . . . . Indentation Experiments . . . . . . . . . . . . . . . . Interlude: Carbon Nanotube Tips . . . . . . . . . . . . Interlude: Thermal Force and Indentation Formation . Interlude: Rim Formation on Polymer Samples . . . . Indentation Kinetics and the Indentation Mechanism . Interlude: Thermo-Nano-Mechanics Without a Heater
229 229 230 232 234 234 236 239
. . . . .
. . . . .
. . . . . . . .
. . . . .
. . . . . . . .
. . . . .
. . . . . . . .
. . . . .
. . . . . . . .
. . . . .
. . . . . . . .
. . . . .
. . . . . . . .
. . . . . . . .
Contents – Volume IV
XXIX
29.5
Thermomechanical Nanowear Testing . . . . . . . . . . . . . . . .
241
29.6 29.6.1 29.6.2
Application to Data-Storage Devices . . . . . . . . . . . . . . . . . Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Scaling Challenges for Nanoindentation of Polymers . . . . . . . .
243 243 245
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
248
30
Applications of Heated Atomic Force Microscope Cantilevers Brent A. Nelson, William P. King . . . . . . . . . . . . . . . . . . .
251
30.1
Introduction . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
251
30.2 30.2.1 30.2.2 30.2.3
Physical and Environmental Sensing . . . . . . . . . . . . Pressure Sensing . . . . . . . . . . . . . . . . . . . . . . . Thermal Conductivity Mapping and Subsurface Imaging . Topographical Detection . . . . . . . . . . . . . . . . . .
. . . .
. . . .
. . . .
. . . .
. . . .
252 252 253 258
30.3 30.3.1 30.3.2 30.3.3 30.3.4
Chemical Sensing Applications . . . . . . . Calorimetry . . . . . . . . . . . . . . . . . Mass Detection . . . . . . . . . . . . . . . Time-of-Flight Scanning Force Microscopy Explosives Detection . . . . . . . . . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
261 261 262 263 264
30.4 30.4.1 30.4.2
Data Storage and Lithography . . . . . . . . . . . . . . . . . . . . Data Storage . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Lithography . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
264 265 269
30.5
Summary and Conclusions . . . . . . . . . . . . . . . . . . . . . .
272
References . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
272
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
. . . . .
Subject Index . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 277
Contents – Volume I
Part I
Scanning Probe Microscopy
1
Dynamic Force Microscopy André Schirmeisen, Boris Anczykowski, Harald Fuchs . . . . . . .
3
Interfacial Force Microscopy: Selected Applications Jack E. Houston . . . . . . . . . . . . . . . . . . . . . . . . . . . .
41
Atomic Force Microscopy with Lateral Modulation Volker Scherer, Michael Reinstädtler, Walter Arnold . . . . . . . .
75
Sensor Technology for Scanning Probe Microscopy Egbert Oesterschulze, Rainer Kassing . . . . . . . . . . . . . . . .
117
Tip Characterization for Dimensional Nanometrology John S. Villarrubia . . . . . . . . . . . . . . . . . . . . . . . . . .
147
2 3 4 5
Part II
Characterization
6
Micro/Nanotribology Studies Using Scanning Probe Microscopy Bharat Bhushan . . . . . . . . . . . . . . . . . . . . . . . . . . . .
171
Visualization of Polymer Structures with Atomic Force Microscopy Sergei Magonov . . . . . . . . . . . . . . . . . . . . . . . . . . . .
207
Displacement and Strain Field Measurements from SPM Images Jürgen Keller, Dietmar Vogel, Andreas Schubert, Bernd Michel . .
253
7 8 9
AFM Characterization of Semiconductor Line Edge Roughness Ndubuisi G. Orji, Martha I. Sanchez, Jay Raja, Theodore V. Vorburger . . . . . . . . . . . . . . . . . . . . . . . . . 277
10
Mechanical Properties of Self-Assembled Organic Monolayers: Experimental Techniques and Modeling Approaches Redhouane Henda . . . . . . . . . . . . . . . . . . . . . . . . . . .
303
XXXII
11 12
Contents – Volume I
Micro-Nano Scale Thermal Imaging Using Scanning Probe Microscopy Li Shi, Arun Majumdar . . . . . . . . . . . . . . . . . . . . . . . .
327
The Science of Beauty on a Small Scale. Nanotechnologies Applied to Cosmetic Science Gustavo Luengo, Frédéric Leroy . . . . . . . . . . . . . . . . . . .
363
Part III Industrial Applications 13 14 15
16
SPM Manipulation and Modifications and Their Storage Applications Sumio Hosaka . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
389
Super Density Optical Data Storage by Near-Field Optics Jun Tominaga . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
429
Capacitance Storage Using a Ferroelectric Medium and a Scanning Capacitance Microscope (SCM) Ryoichi Yamamoto . . . . . . . . . . . . . . . . . . . . . . . . . . .
439
Room-Temperature Single-Electron Devices formed by AFM Nano-Oxidation Process Kazuhiko Matsumoto . . . . . . . . . . . . . . . . . . . . . . . . .
459
Subject Index . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 469
List of Contributors – Volume II
Leon Abelmann Systems and Materials for Information storage group MESA + Research Institute P.O. Box 217, 7500 AE Enschede, The Netherlands e-mail:
[email protected] Maria Allegrini INFM and Dipartimento di Fisica “Entrico Fermi”, Università di Pisa Largo Bruno Pontecorvo 3, I-56127 Pisa, Italy e-mail:
[email protected] Boris Anczykowski nanoAnalytics GmbH, Gievenbecker Weg 11, 48149 Münster, Germany e-mail:
[email protected] Piero Castrataro Scuola Superiore Sant’Anna, Polo Sant’Anna Valdera – CRIM Lab Viale Rinaldo Piaggio, 34, 56025 Pontedera (PI), Italy e-mail:
[email protected] Bernard Cretin Department LPMO, FEMTO-ST Institute, UMR CNRS 6174 32 avenue de l’Observatoire, 25044 Besançon Cedex, France e-mail:
[email protected] Paolo Dario Scuola Superiore Sant’Anna, Polo Sant’Anna Valdera – CRIM Lab Viale Rinaldo Piaggio, 34, 56025 Pontedera (PI), Italy e-mail:
[email protected] Harald Fuchs Center for Nanotechnology (CeNTech) and Institute of Physics University of Münster, Gievenbecker Weg 11, 48149 Münster, Germany e-mail:
[email protected] Paul Girard LAIN, UMR CNRS 5011, CC 082, Université de Montpellier II Place E. Bataillon, 34095 Montpellier Cedex 5, France e-mail:
[email protected]
XXXIV
List of Contributors – Volume II
Hermann Gruber Institute for Biophysics, J. Kepler University Altenbergerstr. 69, A-4040 Linz, Austria e-mail:
[email protected] Pietro Giuseppe Gucciardi CNR-Istituto per i Processi Chimico-Fisici Via La Farina 237, I-98123 Messina, Italy e-mail:
[email protected] Peter Hinterdorfer Institute for Biophysics, J. Kepler University Altenbergerstrasse 69, A-4040 Linz, Austria e-mail:
[email protected] Rainer Kassing University of Kassel Institute for Microstructure Technologies and Analytics, IMA Technological Physics Heinrich-Plett-Str. 40, D-34132 Kassel, Germany e-mail:
[email protected] Yoichi Kawakami Department of Electronic Science, Graduate School of Engineering Kyoto University, Nishikyo-ku, Katsura, 615-8510 Kyoto, Japan e-mail:
[email protected] Ferry Kienberger Institute for Biophysics, J. Kepler University Altenbergerstr. 69, A-4040 Linz, Austria e-mail:
[email protected] Jürgen Kirschner Max-Planck-Institut für Mikrostrukturphysik Weinberg 2, 06120 Halle, Germany e-mail:
[email protected] Andrzej J. Kulik Ecole Polytechnique Fédérale de Lausanne, EPFL – IPMC – NN 1015 Lausanne, Switzerland e-mail: Andrzej.Kulik@epfl.ch Nicole Lawrence (geb. Schwendler) Technische Universität Kaiserslautern Erwin-Schrödinger Strasse, 67663 Kaiserslautern, Germany e-mail:
[email protected]
List of Contributors – Volume II
Małgorzata Lekka The Henryk Niewodniczañski Institute of Nuclear Physics Polish Academy of Sciences Radzikowskiego 152, 31-342 Kraków, Poland e-mail:
[email protected] Arianna Menciassi Scuola Superiore Sant’Anna, Polo Sant’Anna Valdera – CRIM Lab Viale Rinaldo Piaggio, 34, 56025 Pontedera (PI), Italy e-mail:
[email protected] Ruggero Micheletto Department of Electronic Science, Graduate School of Engineering Kyoto University, Nishikyo-ku, Katsura, 615-8510 Kyoto, Japan e-mail:
[email protected] Egbert Oesterschulze Universität Kaiserslautern, Fachbereich Physik Physik und Technologie der Nanostrukturen Erwin-Schrödinger Straße, 67653 Kaiserslautern, Germany e-mail:
[email protected] Ute Rabe Fraunhofer Institute for Nondestructive Testing, IZFP, Bldg. 37 D-66123 Saarbrücken, Germany e-mail:
[email protected] Vittoria Raffa Scuola Superiore Sant’Anna, Polo Sant’Anna Valdera – CRIM Lab Viale Rinaldo Piaggio, 34, 56025 Pontedera (PI), Italy e-mail:
[email protected] Tilman E. Schäffer Center for Nanotechnology (CeNTech) and Institute of Physics University of Münster, Gievenbecker Weg 11, 48149 Münster, Germany e-mail:
[email protected] Uta Schlickum Max-Planck-Institut für Mikrostrukturphysik Weinberg 2, 06120 Halle, Germany e-mail: uta.schlickum@epfl.ch Martin Stark Ecole Polytechnique Fédérale de Lausanne Institut des Sciences et Ingénierie Chimiques Laboratory of Ultrafast Laser Spectroscopy 1015 Lausanne, Switzerland e-mail: Martin.Stark@epfl.ch
XXXV
XXXVI
List of Contributors – Volume II
Robert W. Stark Ludwig-Maximilians-Universität München and Center for NanoScience (CeNS) Dept. Earth and Environmental Sciences, Section Crystallography Theresienstr. 41, 80333 München, Germany e-mail:
[email protected] Alexander N. Titkov Ioffe Physico-Technical Institute, 26 Polytecknicheskaya 194021 St Petersburg, Russia e-mail:
[email protected] Pascal Vairac Department LPMO, FEMTO-ST Institute, UMR CNRS 6174 32 avenue de l’Observatoire, 25044 Besançon Cedex, France e-mail:
[email protected] Arnout van den Bos Systems and Materials for Information storage group MESA + Research Institute P.O. Box 217, 7500 AE Enschede, The Netherlands e-mail:
[email protected] Gunther Wittstock Carl von Ossietzky Universität Oldenburg Carl von Ossietzky Str. 9–11, 26129 Oldenburg, Germany e-mail:
[email protected] Wulf Wulfhekel Max-Planck-Institut für Mikrostrukturphysik Weinberg 2, 06120 Halle, Germany e-mail:
[email protected] Christiane Ziegler Technische Universität Kaiserslautern Erwin-Schrödinger Strasse, 67663 Kaiserslautern, Germany e-mail:
[email protected]
List of Contributors – Volume III
Maria Allegrini INFM and Dipartimento di Fisica “Enrico Fermi”, Università di Pisa Largo Bruno Pontecorvo 3, 56127 Pisa, Italy e-mail:
[email protected] Friedrich Aumayr Institut für Allgemeine Physik, Technische Universität Wien Wiedner Hauptstraße 8-10/134, A 1040 Wien, Austria e-mail:
[email protected] Bharat Bhushan Nanotribology Laboratory for Information Storage and MEMS/NEMS (NLIM) 650 Ackerman Road, Suite 255, The Ohio State University Columbus, OH 43202-1107, USA e-mail:
[email protected] Zachary Burton Shell Global Solutions (US) Inc. 3333 Highway 6 South, Houston, TX 77082-3101, USA e-mail:
[email protected] Renato Buzio National Institute for Physics of Matter INFM Via Dodecaneso 33, 16146 Genova, Italy e-mail: buzio@fisica.unige.it Manfred Drack GrAT Center for Appropriate Technology, Technische Universität Wien Wiedner Hauptstraße 8-10/965, A 1040 Wien, Austria e-mail:
[email protected] Andreas Ebner Institute for Biophysics, J. Kepler University Altenbergerstr. 69, A-4040 Linz, Austria e-mail:
[email protected]
XXXVIII
List of Contributors – Volume III
Friedrich Franek Austrian Center of Competence for Tribology Viktor Kaplan-Straße 2, A 2700 Wiener Neustadt, Austria Institut für Sensor- und Aktuatorsysteme, Technische Universität Wien Floragasse 7/2, A 1040 Wien, Austria e-mail:
[email protected] Luca Gavioli INFM and Dipartimento di Matematica e Fisica Università Cattolica del Sacro Cuore via dei Musei 41, I-25121 Brescia, Italy e-mail:
[email protected] Ille C. Gebeshuber Austrian Center of Competence for Tribology Viktor Kaplan-Straße 2, A 2700 Wiener Neustadt, Austria Institut für Allgemeine Physik, Technische Universität Wien Wiedner Hauptstraße 8-10/134, A 1040 Wien, Austria e-mail:
[email protected] Enrico Gnecco National Center of Competence in Research in Nanoscale Science University of Basel 4056 Basel, Switzerland e-mail:
[email protected] Peter Hinterdorfer Institute for Biophysics, J. Kepler University Altenbergerstr. 69, A-4040 Linz, Austria e-mail:
[email protected] James K. Knudsen 3328 York Bay, Woodbury, MN 55125 e-mail:
[email protected] Alexander V. Kovalev Tribology Department Metal-Polymer Research Institute of Belarus National Academy of Sciences Kirov st. 32A, Gomel, 246652, Belarus e-mail:
[email protected] Massimiliano Labardi INFM, Largo Bruno Pontecorvo 3, 56127 Pisa, Italy e-mail:
[email protected] Tobias Lange Institute of Physiology II Robert-Koch Str. 27b, 48149 Muenster, Germany e-mail:
[email protected]
List of Contributors – Volume III
XXXIX
Ernst Meyer National Center of Competence in Research in Nanoscale Science University of Basel 4056 Basel, Switzerland e-mail:
[email protected] Nikolai K. Myshkin Tribology Department Metal-Polymer Research Institute of Belarus National Academy of Sciences Kirov st. 32A, Gomel, 246652, Belarus e-mail address:
[email protected] Dessy Nikova Institute of Physiology II Robert-Koch Str. 27b, 48149 Muenster, Germany e-mail:
[email protected] Laurent Nony L2MP, Equipe Nanostructuration, Faculté des Sciences de Saint-Jérôme 13397 Marseille, France e-mail:
[email protected] Hans Oberleithner Institute of Physiology II Robert-Koch Str. 27b, 48149 Muenster, Germany e-mail:
[email protected] René M. Overney Department of Chemical Engineering, University of Washington Box 351750, Seattle, WA 98195-1750, USA e-mail:
[email protected] Mark I. Petrokovets Tribology Department Metal-Polymer Research Institute of Belarus National Academy of Sciences Kirov st. 32A, Gomel, 246652, Belarus e-mail:
[email protected] Lev Rapoport Department of Science, Holon Academic Institute of Technology 52 Golomb St., Holon 58102, Israel e-mail:
[email protected] Massimo Sancrotti INFM and Dipartimento di Matematica e Fisica Università Cattolica del Sacro Cuore via dei Musei 41, I-25121 Brescia, Italy Laboratorio TASC-INFM Strada Statale 14, km. 163.5, Basovizza, I-34012 Trieste, Italy e-mail:
[email protected]
XL
List of Contributors – Volume III
Hermann Schillers Institute of Physiology II Robert-Koch Str. 27b, 48149 Muenster, Germany e-mail:
[email protected] Scott Sills Department of Chemical Engineering, University of Washington Box 351750, Seattle, WA 98195-1750, USA e-mail:
[email protected] Oleg Tikhomirov Institute of Solid State Physics, Chernogolovka 142432, Russia INFM, Largo Bruno Pontecorvo 3, 56127 Pisa, Italy e-mail:
[email protected] Ugo Valbusa National Institute for Physics of Matter INFM and Dipartimento di Fisica dell’Università degli Studi di Genova Via Dodecaneso 33, 16146 Genova, Italy e-mail: valbusa@fisica.unige.it Armen Verdyan Department of Science, Holon Academic Institute of Technology 52 Golomb St., Holon 58102, Israel e-mail:
[email protected] Hannspeter Winter Institut für Allgemeine Physik, Technische Universität Wien Wiedner Hauptstraße 8-10/134, A 1040 Wien, Austria e-mail:
[email protected]
List of Contributors – Volume IV
Chunli Bai National Center for Nanoscience and Technology Beijing 100080, P.R. China e-mail:
[email protected] James D. Batteas National Institute of Standards and Technology Surface and Microanalysis Science Division 100 Bureau Drive, Stop 8372, Gaithersburg, MD 20899 e-mail:
[email protected] Bharat Bhushan Nanotribology Laboratory for Information Storage and MEMS/NEMS (NLIM) Ohio State University, Columbus, OH 43210, USA e-mail:
[email protected] U. Dürig IBM Research GmbH, Zurich Research Laboratory Säumerstrasse 4, CH-8803 Rüschlikon, Switzerland e-mail:
[email protected] Fernando García Instituto de Microelectrónica de Madrid, CSIC C/ Isaac Newton 8, 28760, Tres Cantos, Madrid, Spain e-mail:
[email protected] Ricardo García Instituto de Microelectrónica de Madrid, CSIC C/ Isaac Newton 8, 28760, Tres Cantos, Madrid, Spain e-mail:
[email protected] Jayne C. Garno Department of Chemistry, Louisiana State University 232 Choppin Hall, Baton Rouge, LA 70803 e-mail:
[email protected]
XLII
List of Contributors – Volume IV
Christoph Gerber National Competence Center of Research in Nanoscale Science, Basel Klingelbergstrasse 82, CH-4056 Basel, Switzerland e-mail:
[email protected] B. Gotsmann IBM Research GmbH, Zurich Research Laboratory Säumerstrasse 4, CH-8803 Rüschlikon, Switzerland e-mail:
[email protected] Martin Hegner National Competence Center of Research in Nanoscale Science, Basel Klingelbergstrasse 82, CH-4056 Basel, Switzerland e-mail:
[email protected] Albena Ivanisevic Purdue University, Weldon School of Biomedical Engineering 500 Central Drive, West Lafayette, Indiana 47907-2022 e-mail:
[email protected] Joseph M. Kinsella Purdue University, Department of Biomedical Engineering 500 Central Drive, West Lafayette, Indiana 47907-2022 e-mail:
[email protected] Hans Peter Lang National Competence Center of Research in Nanoscale Science, Basel Klingelbergstrasse 82, CH-4056 Basel, Switzerland IBM Zurich Research Laboratory, Säumerstrasse 4, CH-8803 Rüschlikon, Switzerland e-mail:
[email protected] Carmen LaTorre Owens Corning, Insulating Systems Business 2790 Columbus Road, Route 16 (Bldg 20-1), Granville, OH 43023, USA e-mail:
[email protected] William P. King Woodruff School of Mechanical Engineering, Georgia Institute of Technology 771 Ferst Drive N.W., Atlanta, GA 30332-0405 e-mail:
[email protected] Brent A. Nelson Woodruff School of Mechanical Engineering, Georgia Institute of Technology 771 Ferst Drive N.W., Atlanta, GA 30332-0405 e-mail:
[email protected]
List of Contributors – Volume IV
Marta Tello Instituto de Microelectrónica de Madrid, CSIC C/ Isaac Newton 8, 28760, Tres Cantos, Madrid, Spain e-mail:
[email protected] Chen Wang National Center for Nanoscience and Technology Beijing 100080, P.R. China e-mail:
[email protected]
XLIII
1 Higher Harmonics in Dynamic Atomic Force Microscopy Robert W. Stark · Martin Stark
1.1 Introduction Aside from its ability to image and visualize the specimen, atomic force microscopy (AFM) offers the potential to perform a wide variety of quantitative measurements. For example, indenting the surface of a polymer with the tip allows us to characterize its viscoelastic properties, while long-range electrostatic forces can be used to detect the number of charges stored in a semiconductor nanostructure. In AFM, a force (from the sample) acting on the sensing tip of the atomic force microscope will influence the motion of the cantilever that the tip is attached to. The motion of this cantilever is observed and quantified by a detection system, and eventually parameterized into the quantities of interest. Fundamentally, all AFM is dynamic: the motion of the tip varies with time under the influence of the forces acting upon it. However, parameterization of the measurements is required to establish a link between the measurements and the physical quantities of interest. It is precisely this task – the establishment of a link between the detected motion of the lever and the physical property of the sample – that gives rise to the wide variety of AFM modes currently employed. Amplitude modulation (also known as tapping mode or intermittent contact mode) has become a standard technique used to perform surface imaging by dynamic AFM under ambient conditions [1]. In this imaging mode, the cantilever is excited at its fundamental resonance to an oscillation amplitude of typically 10 nm to 100 nm. The interaction between the tip and the sample limits the oscillatory amplitude. In order to track the surface profile, feedback circuitry controls the relative position of the tip to the sample during scanning, keeping the oscillation amplitude constant. Phase imaging [2] (the acquisition of the phase lag between the driving force and the cantilever response) has proven to be a powerful method of characterizing mechanical and chemical surface properties. Specific chemical information is obtained by employing functionalized tips [3]. Apart from the topography, the average deflection is recorded together with the amplitude and the phase of the cantilever motion during conventional phase imaging. This additional data corresponds to the first two Fourier coefficients of the AFM signal: the zeroth harmonic (DC component) and the amplitude and phase of the first harmonic. However, since the amplitude signal is used for feedback in order to track the surface topography, this signal is equivalent to the control error and does not contain novel information. The phase signal carries information on the local energy dissipation [4], which
2
R.W. Stark · M. Stark
is determined by chemical [3] and mechanical surface properties [2, 5]. A precise interpretation of the phase signal remains difficult, however, since it includes contributions from the local topography [6]. The slowly varying part of the signal spectrum (DC) is also referred to as the “tapping mode deflection”. This DC-signal encodes the time-averaged interaction force [7–10]. More information is available from analyzing further signal components or the entire spectral response. Although the free cantilever can be approximated by a onedimensional harmonic oscillator for many applications [11], the broadband signal formation can only be understood by taking higher eigenmodes into account (see Fig. 1.1). When approaching the surface, the oscillation amplitude is confined by the sample surface on one side, creating an analogy to the “impact oscillators” studied in structural mechanics [12–15]. The confinement induced by the sample surface acts as a barrier, and it this is defined by the attractive and repulsive surface forces (by the chemical and mechanical properties of the sample) [16–18]. Despite the nonlinear interaction, tip oscillation remains periodic under stationary measurement conditions [19]. As a consequence, any influences from nonlinearities will appear as higher harmonics of the fundamental frequency [4, 20–27]. Deviations from the purely sinusoidal behavior of the oscillation can also arise from dissipative effects. The tip approaches and retracts from the surface during a single oscillation cycle. Energy dissipation causes hysteresis of the tip motion and introduces higher Fourier components [22, 26, 28]. The signal amplitudes of the higher harmonics of a periodic signal generated by a nonlinear system can therefore be used to infer the characteristics of the nonlinearity by balancing the harmonics of the system input and the output [29–32]. Furthermore, it is important to note that the microcantilever is an extended structure with a complex dynamical behavior [33–36]. The cantilever can undergo a variety of oscillatory motions that are related to the flexural, torsional and bending modes of the structure [37–42]. Multimodal AFM techniques take advantage of the resonance structure of the cantilever [43–45]. The
Fig. 1.1. Scheme of higher harmonics generation in atomic force microscopy. There are two aspects that are important for the spectral characteristics of the AFM signal: the nonlinearity of the tip–sample interaction, and the multiple resonances of the cantilever. Due to the nonlinear tip–sample interaction, the force signal is distorted. Higher harmonics of the driving frequency prevail in the spectrum, which is modified by the transfer characteristics of the cantilever. The spectral characteristics are therefore closely related to the tip–sample forces, such as the mechanical, electrostatic and van der Waals forces
1 Higher Harmonics in Dynamic Atomic Force Microscopy
3
resonant frequencies of the higher eigenmodes of commercial AFM cantilevers are usually not integer multiples of the fundamental resonance frequency [34, 41], although harmonic cantilevers modified to purpose have recently been introduced [46]. Two key elements can be identified that contribute to a deviation of the cantilever dynamics from a simple harmonic oscillator: firstly, the non-linearity introduces harmonics (integer multiples of the fundamental oscillation frequency) into the signal spectrum; secondly, higher eigenmodes of the cantilever can be excited (1.1). One important source of higher harmonic generation – electrostatic force – was exploited very early in the development of Kelvin probe force microscopy [47–50]. The attractive force due to a contact potential difference ∆φ between a tip and a sample separated by a distance D is given by Fel (D) =
1 dC ∆φ2 , 2 dD
(1.1)
where C is the capacitance of the tip–sample system. An AC voltage UAC with a frequency ω and a DC (ω = w) offset UDC is applied between tip and sample for potential imaging in Kelvin probe force microscopy. The electrostatic force is then Fel (D) =
1 dC [∆φ − UDC − UAC sin(ωt)]2 . 2 dD
(1.2)
This leads to spectral force components at the harmonic frequencies DC, ω and 2ω: 1 dC 1 2 2 (1.3) FDC (D) = (∆φ − UDC ) + UAC , 2 dD 2 dC Fω (D) = − (1.4) [(∆φ − UDC ) UAC sin(ωt)] dD and F2ω (D) =
1 dC 2 U cos(2ωt) . 4 dD AC
(1.5)
This 2ω component can be used to compensate for the DC potential offset caused by UAC in (1.3) [51]. In an electrolyte, the electrostatic force between tip and sample separated by a distance D follows an exponential law: Fel (D) = Fmax e−D/λ ,
(1.6)
with a characteristic decay length (Debeye length) λ that depends upon the electrolyte concentration. This nonlinear electrostatic force is thought to contribute to the generation of higher harmonics [52]. The following chapter emphasizes the nature of the micromechanical cantilever as a distributed parameter system. The assumption herein is that the cantilever is a geometrically extended structure with an infinite number of eigenfrequencies with corresponding modal shapes (eigenvectors). For theoretical investigations of dynamic AFM, often only the fundamental mode is taken into account, neglecting higher modes. This single degree of freedom (SDOF) approximation permits the
R.W. Stark · M. Stark
4
prediction of basic features of nonlinear dynamics, such as the existence of different oscillatory states [53, 54], the phase lag between driving force and system response [4], or the pressure at the contact area [55]. In an SDOF model with an external force F(t) and state variables of tip displacement x and velocity x˙ x(t) ¨ +
ω0 x(t) ˙ + ω20 x(t) = ω20 F(t) k , Q
(1.7)
the cantilever is fully characterized by its angular resonant frequency ω0 , the spring constant k, and the quality factor Q. The effective mass m is determined by m = k/ω20 . The quality factor is related to the damping γ by Q = 1/(2γ) and can be understood as the amplification factor of an excitation Ad at a resonance ω = ω0 . In this case the oscillation amplitude is given by A0 = Q Ad . In the state space form (1.7) can be rewritten as 2 0 1 0 ω0 x˙ = F(t) , (1.8) x+ 1 k −ω20 −ω0 Q A
b
introducing the state vector x = [x, x] ˙ T , the system matrix A and the input vector b. Generally speaking, the SDOF approximation holds as long as there are only small contributions to the system dynamics at frequencies higher than the fundamental resonance frequency [56]. However, the approximation completely fails to predict the system characteristics at higher frequencies such as those of higher harmonics or of a chaotic response. Obviously, the SDOF approximation does not account for higher resonances of the cantilever. Additionally, there is a second feature of the distributed parameter system that is not present in the SDOF model: a distributed system can exhibit transmission minima (the cantilever can act as a notch filter that strongly suppresses any dynamics at specific frequencies). This effect has been described as a “dynamically frozen cantilever” [57]. In the following, a multiple degree of freedom (MDOF) state space model of an AFM cantilever interacting with the specimen surface is developed. This approach allows us to use an identical model to investigate the characteristics of both freely vibrating and surface-coupled cantilevers. Additionally, this model provides a direct theoretical reason for the generation of higher harmonics from the nonlinearity of the contact between the tip and the sample in tapping mode AFM. The theoretical results are corroborated by experimental data. Analysis of the higher harmonics of the excitations enables us to differentiate between different materials.
1.2 Multimodal Model of the Microcantilever 1.2.1 Overview There are several strategies that could be used to account for the higher order modes of the cantilever. A straightforward approach can be obtained through finite element [41,
1 Higher Harmonics in Dynamic Atomic Force Microscopy
5
58–61] or finite difference analysis [62] of the oscillating cantilever. In this case, the full geometry of the cantilever must be modeled using numerical simulations. Unfortunately, such simulations are highly intensive. However, the computational effort required can be reduced by taking into account only the vibration modes that significantly contribute to the dynamics. This leads to a truncated model consisting of only a limited number of eigenmodes. This simple mode truncation, however, has an important drawback: the exact frequencies of the transmission minima also depend upon the contributions from higher eigenmodes. Thus, a truncation of the model causes the frequencies of the transmission minima to be shifted to higher frequencies [63,64]. However, since the exact frequency of the transmission minima is of minor importance to the understanding of the generation of higher harmonics, we will neglect this effect in the following. The interaction of a silicon tip with a glass surface was modeled for the analytical and numerical calculations. A rectangular silicon cantilever with an idealized optical detection scheme was assumed. A model with N = 3 modes was used in the numerical simulation of nonlinear dynamics, and a model with N = 5 modes was used for linearized analysis. The parameters used are indicated in Table 1.1. Table 1.1. Parameters used to simulate the generation of higher harmonics in atomic force microscopy. There are two aspects that are important for the spectral characteristics of the AFM signal: the nonlinearity of the tip–sample interaction, and the multiple resonances of the force sensor. The interplay between the various tip–sample forces and the spectral characteristics is currently being researched Resonant Spring Modal Young’s Poisson Young’s Poisson Tip Hamaker frequency constant quality Modu- ratio Modulus ratio for radius constant factor lus tip for tip sample sample
Interatomic distance parameter
ω0
a0
normalized
k
Qn
10 N/m 200
Et
νt
129 GPa 0.28
Es 70 GPa
νs 0.17
R
H
20 nm 6.4
×10−20
J 0.166 nm
1.2.2 Modal Analysis As a first step, a modal analysis provides the geometrical shape of the eigenmodes and the corresponding resonant frequencies of the cantilever. These are the most important input parameters for the numerical simulation of the temporal evolution of the system. The advantage of such a modal analysis is that the approach is feasible for arbitrary structures, and it is common engineering practice [65]. For more complicated cantilever geometries, the eigenvalues and eigenvectors can be obtained from a finite element analysis [65, 66]. As a generic and instructive example, higher harmonic generation resulting from the tip–sample interaction will be discussed for the case of a rectangular
R.W. Stark · M. Stark
6
AFM cantilever. Together with further simplifications, such as modal damping and external forcing at the tip, an explicit analytical solution can be obtained for the partial differential equation. These solutions will be used as parameters in the subsequent numerical analysis. The equation of motion for the flexural vibrations of a freely vibrating and undamped cantilever beam can be approximated by the Euler–Bernoulli equation [67] EI
∂ 2 z(ξ, t) ∂ 4 z(ξ, t) + m =0, ∂ξ 4 ∂t 2
(1.9)
with vertical displacement z(ξ, t), normalized position ξ ∈ [0, 1] along the cantilever, time t, flexural stiffness E I, and constant mass per unit length m. The resonant frequency of the nth eigenmode ωn is related to the respective eigenvalues kn by ω2n = (kn )4 E I/m .
(1.10)
The eigenvectors (modal shapes) ϕ(ξ) are determined by the boundary conditions. The cantilever is clamped at ξ = 0. The boundary conditions are ϕ(w) = 0 for the displacement and ϕ (w) = 0 for the deflection slope. At ξ = 1 the cantilever is free, there are no external torques or shear forces; ϕ (x) = 0 and ϕ (1) = 0, respectively. The eigenvalues can be obtained from the characteristic equation cos kn cosh kn = −1 .
(1.11)
Here, the asymptotic solution kn(a) = (n − 12 )π of (1.11) is a useful approximation for higher modes (n > 3). If the tip is in contact with the surface but can slide laterally (clamped–pinned beam: ϕ(x) = 0 and ϕ (x) = 0), one correspondingly obtains cos kn sinh kn + sin kn cosh kn = 0 .
(1.12)
The eigenvectors of the free cantilever are given by: ϕn (ξ) = cos kn ξ − cosh kn ξ −
cos kn + cosh kn (sin kn ξ − sinh kn ξ) . sin kn + sinh kn
(1.13)
The first four flexural eigenmodes are illustrated in Fig. 1.2. By assuming nonclassical boundary conditions through the addition of translational and rotational springs at the clamped end instead of the rigid constraints ϕ(w) = ϕ (w) = 0, the accuracy of the theoretical calculations can be increased still further [68]. To simplify the problem, we assume that the massless tip is located at the free end at ξ = 1. Additionally, we assume that the laser light used to detect cantilever movement is focused on the free end, and that all forces, such as magnetic actuation and tip–sample forces, act on the free end. With these assumptions, the driving and the tip–sample forces are collocated with the deflection sensing system (ξdrive = ξsens = ξtip ). This avoids difficulties such as nonminimum phase response or time delays that can occur in noncollocated systems [69]. A more realistic analysis of optical detection is discussed in Sect. 1.2.8. From the modal bending shape we obtain the modal displacement ϕn (ξ) and the modal deflection angle ϕn (ξ), which is an idealized light lever readout with an
1 Higher Harmonics in Dynamic Atomic Force Microscopy
7
Fig. 1.2. Illustration of the first four flexural eigenmodes of a freely vibrating rectangular cantilever beam
infinitely small laser spot. These modal parameters can be understood as coupling coefficients. The modal displacement describes the coupling efficiency of a tip–sample force to the corresponding mode, and the modal deflection describes the coupling of the respective mode to the sensing system. As we will see in Sect. 1.2.4, there are subtle differences between the transfer characteristics of a deflection angle readout (light lever) as compared to a position readout (tip displacement and interferometer). 1.2.3 Tip–Sample Interaction DMT Model The interaction between tip and sample is determined by the attractive and repulsive surface potentials. The distance between tip and sample is D = z s + z. The scalar z is the tip deflection and the scalar z s is the distance between the undeflected cantilever and the sample. Van der Waals forces dominate the interaction in the attractive regime (D ≥ a0 ). In the repulsive regime (D < a0 ), the tip–sample forces are calculated from the Derjaguin–Muller–Toporov (DMT) model [70]. The DMT model describes a situation where the energy dissipation due to tip–sample contact is negligible. To avoid an unphysical divergence, the parameter a0 is introduced, corresponding to the interatomic distance [54]. The tip sample forces are given by ⎧ 2 D ≥ a0 ⎨ −HR/ 6 (z s + z) Fts (z) = , (1.14) √ ⎩ −HR/6a2 + 4 E ∗ R (a0 − z s − z)3/2 D < a0 0 3 where H is the Hamaker constant and R the radius of the tip. The effective contact −1
stiffness is calculated from E ∗ = 1 − νt2 /E t + 1 − νs2 /E s , where E t and E s are the respective elastic moduli and νt and νs the Poisson ratios of the tip and the sample, respectively. It should be mentioned that the choice of bulk material parameters for the nanoscale simulations can only be a crude estimation. It has been shown that hard-
R.W. Stark · M. Stark
8
ness of a material at the nanometer scale can differ significantly from its microhardness [71]. Additionally, one should bear in mind that silicon tips are typically covered by a silicon oxide layer [72]. Nevertheless, numerical simulations based on these bulk parameters provide useful predictions of the system dynamics. For very small oscillations around an equilibrium position z 0 , (1.14) can be linearized [34], leading to D ≥ a0 −HR/ 3 (z s + z 0 )3 ∂ ∗ √ = . (1.15) kts = − Fts (z) ∗ 1/2 ∂z 2E R (a0 − z s − z 0 ) D < a0 z=z 0 In the following sections, the contact stiffness kts∗ is normalized to the cantilever spring constant k by kˆ ts = kts∗ /k. Electrostatic Forces Aside from the attractive van der Waals forces, the electrostatic interaction between the tip and the sample is another source of higher harmonics generation. From (1.1), it is clear that a nonlinear electrostatic interaction is also present during imaging due to a contact potential difference, since dC(D)/ dD is not linear. For smooth surfaces the electrical capacitance between a sphere with radius R and a plane is given for D/R 1 by R θ , (1.16) C(D) ≈ 2πε0 R ln + 1.843 + D 63 with the parameter θ ∈ [0, 1], and ε0 being the electrical permittivity of the medium [73]. Thus, within the limit of small oscillation amplitudes, the electrostatic force (1.1) acting at the tip is reciprocally proportional to D [74] with Fel (D) = −
πε0 R ∆φ2 . D
(1.17)
A slight roughness of tip or sample can prevent divergence in (1.17) [73]. For large distances D/R 1 [74], the electrostatic force is Fel (D) = −
πε0 R2 ∆φ2 . D2
(1.18)
The attractive van der Waals force for the plane sphere configuration exhibits a similar distance relationship FvdW (D) = −
HR . 6D2
(1.19)
In the limit D/R 1 the attractive electrostatic and van der Waals forces exhibit the same force vs. distance relationship [75]. Thus, control of the potential ∆φ between tip and sample is essential in order to distinguish between electrostatic and van der Waals forces in a mechanical AFM experiment.
1 Higher Harmonics in Dynamic Atomic Force Microscopy
9
1.2.4 State Space Formulation In the following, a multiple degree of freedom (MDOF) model of the cantilever will be developed, which employs the state space formalism. The cantilever is conceived as a linear time-invariant system that is subject to a nonlinear output feedback caused by tip–sample interaction, as illustrated in Fig. 1.3. This feedback perspective of dynamic AFM [30,76] allows for a numerically efficient investigation of the dynamics of the system [9, 77]. The input (1) accounts for external forcing at the free end of the cantilever as well as for the tip–sample forces. External forces at input (1) can be experimentally realized by a magnetic actuation of the cantilever, for example. Further system inputs such as the displacement of the sample (input(2)) or the cantilever base (input (3)) will not be discussed. Output (1) is the deflection of the free end of the cantilever (the physical displacement of the tip) and output (2) corresponds to the light lever readout of the system (the signal that is usually measured). The state space form of the equations of motion of the cantilever with N degrees of freedom (eigenmodes) is x˙ = Ax + bu , y = Cx
(1.20)
analogous to the SDOF formulation introduced in (1.8). The time-dependent state vector x = (x1 , x2 , . . . ) = (xn=1 , ∂t xn=1 , . . . ) contains the generalized displacements and velocities of the individual eigenmodes. The 2N × 2N matrix A is the system matrix, b is the input vector, and the scalar u is the force input. In the case of
Fig. 1.3. (a) Schematics of dynamic atomic force microscopy. Commonly used inputs and outputs of the dynamical system are indicated. The system can be accessed by applying forces u(t) directly onto the free end of the cantilever (input 1), such as the tip–sample interaction or external actuation. Alternative inputs include base excitation of the sample (input 2) or excitation of the cantilever support (input 3). The tip deflection z tip (t) (output 1) determines the tip–sample interaction force. However, often this output cannot be observed directly. Most commonly, the angle of the cantilever deflection is read out using an optical lever detection scheme determining the difference signal S− (t) (output 2). (b) Graphical representation of the dynamic system. The cantilever is represented by a linear and time-invariant (LTI) submodel. The tip–sample interaction force is a nonlinear output feedback that depends on the tip position
R.W. Stark · M. Stark
10
multiple inputs, the vector b and the scalar u transform into a matrix and a vector, respectively. The output vector y consists of the tip displacement output y1 and the photodiode signal output y2 , which are linear combinations of the system states xi . The corresponding weights are given by the output matrix C. Note that, in comparison to the structure of (1.8), it is now necessary to introduce an output matrix in order to distinguish between different outputs. There is no feed-through between the input and the outputs. The modal quality factors are usually larger than 100 under ambient conditions. This means that there is only a very weak intrinsic damping and a weak damping due to the surrounding gas. Thus, we can assume a modal damping which leads to a decoupling of eigenmodes that implies normal modes: the modal contributions oscillate in phase. The system matrix A has a very simple structure and consists of the 2 × 2 submatrices of the eigenmodes along the main diagonal. In other words, the cantilever bending line is stationary for normal modes. This is in contrast to nonmodal damping, which leads to complex mode shapes where the phase angle varies along the structure [66]. Such “traveling” or complex modes can occur in liquids due to viscous damping in the fluid (see, for example, Fig. 8 in [78]). The submatrices are constructed from the eigenfrequency ω n = ωn /ω1 and the modal quality factor Q n , which is related to the modal damping γn = 1/(2Q n ). The eigenfrequencies are normalized to the fundamental resonant frequency of the cantilever. The dynamics of the nth mode can be described by the modal state vector xn , the system matrix An , and the input vector bn , using x xn = n , x˙n An =
0 1 ωn /Q n − ωn2 −
0 bn = ϕn (1)/Mn
,
(1.21)
.
The modal state vector simply consists of the modal displacement and velocity. The modal system matrix corresponds to that of a single degree of freedom harmonic oscillator. The first component of the input vector bn is zero, while the second component describes the coupling of an input force to the eigenmode. It is given by the respective modal displacement ϕn at the tip position ξtip = 1, weighted with the 1 respective generalized modal masses Mn = 0 mϕn (ξ)2 dξ. Without restriction the mass density is normalized to Mi = m = 1. The dynamics of the N degrees-of-freedom system is thus given by ⎤ ⎡ A1 x˙1 ⎢ x˙2 ⎥ ⎢ 0 ⎢ . ⎥=⎢ . ⎣ . ⎦ ⎣ . . . ⎡
x˙ N
⎤⎡ ⎤ ⎡ ⎤ x1 b1 ··· 0 · · · 0 ⎥ ⎢ x2 ⎥ ⎢ b2 ⎥ ⎥⎢ . ⎥ + ⎢ . ⎥u . .. ⎦⎣ . ⎦ ⎣ . ⎦ . . . 0 0 AN xN bN 0 A2 .. .
(1.22)
1 Higher Harmonics in Dynamic Atomic Force Microscopy
11
The output matrix C describes the combination of the system states yielding the output vector with the tip displacement y1 and the deflection readout y2 . For the individual eigenmodes, the contribution to the total output is given by ϕn (ξtip ) 0 . (1.23) Cn = ϕn (ξsens ) 0 Here, ξtip = 1 and ξsens = 1 are the positions of the tip and the detection laser along the cantilever, respectively. The modal bending shapes are given by (1.13). This leads to the system output
y1 y2
⎡
⎤ x1 ⎢ x2 ⎥ ⎥ = C1 C2 · · · C N ⎢ ⎣ .. ⎦ . .
(1.24)
xN It is advantageous to normalize the output channels to the respective frequency response at ω = 0 (DC) by yˆ1 y /yDC = 1 1DC . (1.25) yˆ2 y2 /y2 The normalized deflection output yˆ1 leads to a normalized quasi-static spring constant for the cantilever, kˆ cant = 1. Normalization of the light lever sensor, yˆ2 , reflects the usual quasi-static calibration of the photodiode response from a force vs. displacement curve on a hard sample. The nonlinear interaction between tip and sample can be modeled as an output feedback. The tip displacement is fed back to input (1) through the interaction force Fts ( yˆ1 ). Modeling of the so-called active Q-control is straightforward in this model. For the standard time-delay type of Qcontrol, output yˆ2 is fed back to input (1) with a time delay ∆t and amplified by a gain factor K . Finally, it is worth mentioning that the modes n > N are neglected although they also contribute to the low-frequency response [79]. Additionally, process and measurement noise such as thermomechanical noise, electronic 1/ f noise or shot noise will also be present in the system. 1.2.5 Dynamics: Linearized Tip–Sample Interaction In order to understand the frequency shifts due to attractive or repulsive forces in the light of a MDOF model, it is useful to discuss the case of very small oscillations first. In this situation, we can linearize the tip–sample interaction (1.15). The output feedback is directly proportional to the system’s position output (1). Thus, the elastic surface properties can be conceived as a proportional feedback with a gain parameter kˆ ts . Correspondingly, a dissipative interaction due to viscous sample properties could be represented by a differential controller. For brevity, dissipative tip sample interaction or other time-dependent interaction forces will not be discussed.
12
R.W. Stark · M. Stark
The influence of the tip–sample interaction on the amplitude and the phase response of the system described by (1.22) to (1.24) is illustrated in the Bode plots in Fig. 1.4a. The linearized van der Waals interaction corresponds to a spring with a negative force constant. This leads to a softening of the dynamic system and a corresponding redshift of the resonant frequencies (dash-dotted) in comparison to the freely oscillating cantilever (solid). In contrast, a repulsive tip–sample interaction corresponds to a spring with a positive spring constant. This interaction hardens the system, which results in a blueshift of the resonant frequencies (dashed) [11]. It is important to note that the resonant frequencies depend on the gain factor of the output feedback. However, they are not affected by the choice of the output channel. In contrast, compared to the light lever output (2), the frequencies of the transmission minima are different for the position output (1). The relative frequency shift of the higher eigenmodes is of course smaller than that of the fundamental mode because the frequency shift depends upon the stiffness ratio kˆ ts /m ωˆ 2n , which rapidly decreases with an increasing mode number n. For a very stiff tip–sample contact with kˆ ts = 105 , the system approximately corresponds to a cantilever with its end pinned to the sample surface (Fig. 1.4). The resonant frequencies of the stiff system – seen in the light lever output (2) – correspond to the frequencies of the transmission minima of the displacement output of the free system. This is not surprising, since the poles (resonances) of a constrained system generally correspond to the zeros (antiresonances) of the free system [80]. It is remarkable that the displacement output (1) exhibits a flat amplitude response, whereas in output (2) the resonances remain detectable. In the constrained system,
Fig. 1.4. Bode plot (frequency response) of the cantilever. (a) Position output and (b) idealized light lever readout. The frequency response of the free cantilever is indicated by the solid line. Moderately attractive and repulsive interaction forces shift the resonances to lower and higher frequencies respectively (dashed, dash-dotted). Note that the respective resonance frequencies are the same for both outputs, whereas the transmission minima depend upon the output channel. A strong surface coupling (kts = 105 ) leads to a flat transfer function with a small gain in the position output (a). The system resonances are still visible in the photodiode signal
1 Higher Harmonics in Dynamic Atomic Force Microscopy
13
poles and zeros cancel for output (1), but not for output (2). A physical interpretation is straightforward: the cantilever was modeled as a beam that is actuated by a force at the free end. However, there is now an additional stiff spring attached to the free end which directly counteracts an external driving force. These examples clearly illustrate that a very precise definition of the system inputs and outputs is essential. With the actuation directly at the tip position, there are no measurable dynamics of the tip displacement, whereas a rich structure of resonances and transmission minima can be observed in the light lever output in the case of a surface-coupled cantilever. Physically, this means that there are also different system transfer characteristics, depending on the measurement system. The employment of a light lever readout will provide dynamic characteristics that are different to those from interferometric detection. In order to tailor the system dynamics to specific experimental or control engineering needs, it is also possible to combine a light lever detection with an interferometric detection. For feedback purposes, a linear combination of the signals obtained from a light lever and an interferometer can be advantageous. In robotics, such linear combinations of position and deflection angle detection are used in order to avoid undesired system dynamics such as an unwanted nonminimum phase response of single flexible effectors [69,81]. 1.2.6 Poles and Zeros ∞ The Laplace transformation G(s) = 0 e−st g (t) dt is a convenient tool for the analysis of dynamic systems. The main advantage of the Laplace transformation is the simple calculation of integrals and derivatives with respect to time, which become multiplications and divisions. Thus, differential equations transform into polynomial equations, which are easier to solve. The system output is calculated by convolving the system’s impulse response with the input signal. System characteristics such as resonances, transmission zeros, damping and system stability are conveniently illustrated in the Laplace domain in the so-called pole zero and root locus maps. In the following we will discuss the influence of tip–sample interactions on the system dynamics in the Laplace plane. For the position output (1) of the dynamic system given by (1.22) and (1.24), the state space model can be rewritten as a rational transfer function G(s) =
n
N ϕn ξtip ϕn ξtip = . s2 + ωn s/Q n + ω2n n=1
(1.26)
Thus, the transfer function has the form G(s) =
Z(s) , P(s)
(1.27)
where the denominator P(s) and the numerator Z(s) are polynomials of the complex frequency variable s = iω. This means that the numerator and denominator can be factorized. The roots of P(s) and Z(s) are referred to as poles and zeros, respectively.
14
R.W. Stark · M. Stark
The transfer function can be understood as a complex landscape in the Laplace plane, introducing a real part s = σ +iω. Upon plotting the magnitude of the Laplace transform function |G(s)|, the landscape consists of sharp peaks (poles) and valleys (zeros), as illustrated in Fig. 1.5a. The complex Laplace transform function diverges at the poles and equals zero at the zeros. On a logarithmic scale, the zeros appear as sharp peaks in the negative direction. The amplitude response of the system can be determined from a cross-section through this landscape along the imaginary axis Fig. 1.5b. A projection of the landscape onto the Laplace plane is shown in Fig. 1.5c. Note that, for the cantilever model, the poles and zeros are located in the left half plane, very close to the imaginary axis. Usually, poles and zeros are indicated in the so-called pole zero map as illustrated in Fig. 1.5d. Here, poles are usually marked by crosses, zeros are indicated by open circles. The circles of equal frequency and the lines of equal damping are also indicated. Poles in the left half of the plane have
Fig. 1.5. Illustration of the transfer function G(s) for the dynamics of a microcantilever in the Laplace plane. (a) The magnitude log10 (|G(s)|) as a surface plot on a logarithmic scale. The transfer function diverges at the poles. (b) The frequency response is obtained by a cross-section through the landscape along the imaginary axis. (c) Contour plot of the landscape (a). (d) The pole zero map is obtained from the contour plot by omitting the contour lines. Poles are visualized with crosses, zeros with circles. The dashed lines specify the lines of equal damping as indicated, while the dashed semi circles indicate the locations of equal frequency
1 Higher Harmonics in Dynamic Atomic Force Microscopy
15
a positive damping and are thus stable. In contrast, poles in the right half of the plane exhibit negative damping and are instable. Similarly, the location of the zeros in the Laplace plane is important to the system’s dynamics. Zeros in the left half of the plane can translate into minima in the amplitude response, whereas zeros in the right half of the plane indicate a nonminimum phase response. An additional feedback can manipulate the location of the poles in the complex plane. It also can add or suppress poles. This means that by adding a feedback circuitry such as Q-control, the damping of the system can be reduced or increased and the resonant frequency can be changed. The system zeros are not affected by the feedback, as they depend on the actuators and the sensors of the system. For atomic force microscopy, this means that the system dynamics critically depend on the actuation design of the cantilever and on the deflection sensor system. When a feedback with time delay is added, as for example for the time-delay Q-control [82, 83], the transfer function G(s) ceases to be a rational function, and the mathematical analysis becomes more complicated. A root locus map in the Laplace plane enables a very compact representation of the migration of the system’s poles caused by an additional feedback circuit imposed by the tip–sample forces. The map in Fig. 1.6 visualizes the variations in eigenfrequency and damping in response to a varying effective tip–sample stiffness kˆˆ ts . Here, poles (crosses) and zeros (circles) are shown that belong to the subsystem for the signal flow from input (1) to tip position output (1). For a free cantilever, all of the poles are located in the left half of the plane, and the dynamic system is stable. For the truncated model of a free cantilever, the number of zeros n zero is determined by the number of poles n poles = 2N with n zero = n poles − 2. For the collocated actuation and sensing system, the poles and zeros alternate in the frequency response. Such a collocated configuration of tip and light lever readout is generally desirable in AFM. For an in-depth discussion of the roles of poles and zeros and the collocation of the sensor and the actuator in mechanical systems, see [69, 80, 81]. The zeros are independent from kˆ ts and remain stationary. In the single degree of freedom approximation (N = 1), the dynamic system in (1.8) does not have any zeros. In this case, the resonant frequency diverges to infinity with increasing tip–sample stiffness. This is the reason why the single degree of freedom approximation performs only poorly describes contact mode AFM and completely fails to describe atomic force acoustic microscopy. The migration path of the poles towards the zeros is indicated in Fig. 1.6a for a tip–sample stiffness kˆ ts > 0. For an infinite contact stiffness, the poles and zeros cancel, except for the conjugate complex highest order poles, which diverge. The arrows indicate the direction of migration for an increasing kˆ ts . As can be seen in Fig. 1.6, the poles migrate along bent lines and not along the lines of equal damping. This means that the modal damping can vary substantially depending upon the tip–sample contact. In Fig. 1.6b, the migration of the poles is illustrated for kˆ ts < 0. The arrow indicates the direction of migration for increasing kˆ ts . The poles now migrate towards zeros with lower frequencies. For kˆ ts < −mω21 = −1, one of the dominant poles is real and positive and the system becomes unstable. Experimentally, this instability is well known as “snap-in” [84]. When a soft cantilever closely approaches the surface,
16
R.W. Stark · M. Stark
Fig. 1.6. Root locus map of the linearized closed loop system from input (1) to output (1). The real axis was stretched significantly in order to emphasize the pole migration. The locations of equal damping are indicated by the radial lines, the circles of equal frequency are strongly stretched and appear as horizontal lines. Poles and zeros are indicated by crosses and circles respectively. (a) The arrows give the direction of the pole migration for increasing kˆ ts > 0. For a repulsive tip–sample interaction, the poles migrate towards the next zero with increasing sample stiffness. The highest order poles of the system diverge to infinity. The zeros remain stationary, as they are independent from the feedback. (b) Pole migration for increasing attractive interaction (decreasing kˆ ts < 0). Here, the dominant pole pair (fundamental resonance) migrates towards the real axis. For kˆ ts < −1 one pole is in the right half of the plane and the system is unstable
the cantilever suddenly bends at a certain distance from the surface due to attractive van der Waals forces. Within the framework of this model, the “snap-in” can be understood as an instability of the closed loop system. 1.2.7 Dynamics: Nonlinear Interaction Nonlinearities in the tip–sample contact lead to the generation of higher harmonics. In this section, the theoretical background is illustrated by numerical simulation results. For the numerical simulation, a rectangular cantilever interacting with the surface as described by the nonlinear force law (1.14) was assumed [77]. The simulations were implemented in Matlab Release 13 and Simulink (The Mathworks Inc., Natick, MA, USA). The parameters are summarized in Table 1.1. Since the AFM signal
1 Higher Harmonics in Dynamic Atomic Force Microscopy
17
strongly depends on the alignment of the detection system (see Sect. 1.2.8), only the position output will be considered in this section. Figure 1.7a shows the simulated evolution of the amplitude and phase of the first harmonic, together with the total harmonic distortion THD and the calculated average force f in relation to the size of the tip–sample gap. The amplitude, phase, and average force exhibit the features predicted by the SDOF approximation as being due to the transition from the low amplitude state to the high amplitude state [11]. The anharmonic contributions in the system output (1) were also calculated. The total −1/2 ∞ −1/2
∞ , where harmonic distortion is defined by THD = n=2 |cn | n=1 |cn | |cn | is the amplitude of the nth harmonic, as obtained by the fast Fourier transform (FFT) algorithm. Thus, the THD is the fraction of power that is contained in the higher harmonics. Far away from the sample, the amplitude of the fundamental oscillation is 2|c1 | = 20 nm and the phase is φ = −90◦ . There is only a very small average attractive force and a very small total harmonic distortion. Approaching z s = 20 nm, the system is still in the net attractive (low amplitude) regime, as can be seen by the net negative interaction force. As the strength of the attractive interaction increases, the THD of the output signal also increases. Between z s = 18.5 nm and z s = 18 nm, the system moves to the high amplitude state (arrows). This transition occurs in the temporal evolution of the phase as well as in the average interaction force. It is also visible in the THD, which increases by 50%. Upon further approach, the dynamics of the system change at z s = 2.8 nm. The THD decreases significantly and recovers
Fig. 1.7. The amplitude and phase of the first harmonic, the total harmonic distortion, and the average tip– sample forces, as obtained from the numeric simulation. The transition from the low amplitude state to the high amplitude state can be identified by the phase jump (arrow). The transition between both states is accompanied by a step in the total harmonic distortion of the position output (THD, arrow). Subharmonics are generated in a small gap z s , which lead to a reduction in the THD (asterisk). The transition from net repulsive to net attractive forces is evident in the average force f (arrow)
18
R.W. Stark · M. Stark
at z s = 1 nm, before dropping to zero. This behavior is either explained by the generation of subharmonics, where spectral power is transferred into subharmonics, or by nonperiodic dynamics, where the power is distributed over the entire spectrum. The characteristic features discussed for the THD of simulated data compare well to those seen experimentally [23, 24, 85]. The evolution of the harmonic signal provides additional information on the tip sample interaction. The results from the numerical simulation are shown in Fig. 1.8a. The harmonics are grouped according to the eigenmode that contributes most to the respective signal. In Fig. 1.8, the DC value |c0 |, also known as the “tapping mode deflection”, is shown together with the FFT amplitudes |c1 | to |c4 |, which are grouped around the fundamental frequency. The absolute value of the static deflection due to the average force |∆z| = | f avg |/k perfectly agrees with the DC value |c0 | of the photodiode signal. Thus, the DC value, which is easy to measure in a standard AFM by low-pass filtering the photodiode signal, is a measure of the average tip–sample force. The group below shows the amplitudes |c5 | to |c13 | around the second eigenmode. The amplitudes of these harmonics drop with the onset of period doubling and recover again before the amplitudes drop to zero. The harmonics grouped around the third mode exhibit a significant jump in the transition from the low amplitude to the high amplitude solution (arrow). The different characteristics of the harmonics associated with a particular eigenmode lead to the idea of parameterizing the anharmonic signal in terms of a modal harmonic distortion, as discussed in Sect. 1.4.3. Complex
Fig. 1.8. Simulated harmonics obtained in the position output. They are grouped together according to the eigenmode that contributes most to the signal. (a) The DC contribution (dashed) is a measure of the average tip–sample interaction force. b The harmonics 5–13 around the second and (c) 13–23 around the third eigenmode. (d) Subharmonics are generated for a small separation between cantilever and sample
1 Higher Harmonics in Dynamic Atomic Force Microscopy
19
dynamics appear for small tip–sample gaps of (z s < 5 nm). The subharmonics ω/2, 3/2ω and 11/2ω are shown in Fig. 1.8a. To further investigate the dynamics, it is instructive to analyze the evolution of the spectrum during an approach. Selected spectra obtained by numerical simulation are displayed in Fig. 1.9. The evolution of the spectrum in the range 0 and 2.5ω0 is illustrated by the spectrogram in Fig. 1.10. Away from the sample surface at z s = 21 nm there is only a weak anharmonic contribution. Closer to the surface, higher harmonics prevail over the entire spectrum (see for example z s = 5.3 nm). At smaller separations, more complicated dynamics can be observed. At z s = 2.4 nm the subharmonics are clearly visible, which indicates period doubling. At z s = 1.38 nm the energy is distributed over the entire spectrum, although the harmonics are pronounced. Finally, at z s = 0.4 nm the tip snaps onto the surface and is not then released. Here again we stress that the results from simulation are consistent with those from experiment for a large variety of phenomena, such as the abrupt increase in the contributions from higher harmonics with the onset of repulsive forces, the generation of subharmonics, as well as the overall evolution of the spectrum when approaching a surface [24, 76]. From the numerical data it is clear that the nonlinear tip sample interaction induces a harmonic distortion of the AFM signal. The higher harmonics are experimentally accessible. Increasing the influence of the nonlinearity further, through either a closer approach to the specimen or increased driving amplitude, causes higher periodicity and even chaos [86–88]. The higher harmonics can be used on-line to quantify the interaction forces, and may even be used as input
Fig. 1.9. Fast Fourier transform (FFT) of the position output at various tip–sample gaps z s . Note the period doubling at z s = 2.4 nm, the irregular spectrum at z s = 1.38 nm, the periodic motion again at z s = 1.3 nm, and the nonperiodic system behavior at z s = 1.1 nm
20
R.W. Stark · M. Stark
Fig. 1.10. (color) Spectrogram of the simulated approach (for decreasing z s ). The color depicts the magnitude of the respective frequency component. The frequency is normalized to the fundamental resonance. Initially, only the fundamental and the second harmonics prevail. At z s ≈ 5 nm, complicated dynamics set in and the amplitudes of intermediate frequencies increase. After a periodic motion (z s = 2.5 nm), period doubling occurs, followed by nonperiodic motion. Within the parameter range for nonperiodic motion there are windows of periodic behavior (see Fig. 1.9 with z s = 1.3 nm for example)
to the feedback loop [89]. Furthermore, the experimental results show that higher eigenmode excitation is an important feature in dynamic AFM. 1.2.8 Optical Readout After discussing the dynamics of the system, we will now address the question how the detection of higher eigenmodes can be optimized. Today, most commercially available atomic force microscopes are equipped with light lever detection (Fig. 1.11). There are two parameters related to this that are relevant to system performance: the diameter and the position of the laser spot [90, 91]. Thus, we will evaluate the influence of adjustments made to the laser spot on the transfer characteristics of the sensing system. In Sect. 1.2.4 we showed that the output vector y is a linear combination of the weighted system states (1.23) and (1.24). From (1.13), we know that ϕn (x) = 2(−1)n . In the general case, the parameters for idealized light lever readout ϕn (x) are replaced by the modal coupling factors cn , which account for the coupling of the individual eigenmodes to the light lever readout. These considerations lead to the output matrix −2 0 2 0 · · · 2(−1) N 0 . (1.28) C= c1 0 c2 0 · · · c N 0 Here, output (1), represented by the first row, is still the tip deflection output as defined in Sect. 1.2.4. The second row accounts for light lever readout with a laser spot of a finite size and an arbitrary adjustment of the laser spot on the cantilever.
1 Higher Harmonics in Dynamic Atomic Force Microscopy
21
Fig. 1.11. Scheme of light lever detection in atomic force microscopy. The inset illustrates illumination by a rectangular laser beam. Reprinted with permission from [96]. Copyright (2004), American Institue of Physics
In the following we will calculate the coefficients ci . To this end, we must consider the reflection of the laser light on the curved cantilever. As we have seen, the geometrical shape of a vibrating cantilever beam can be described by (1.13). A Gaussian beam profile is assumed for the laser beam. The irradiance of the laser beam is (ξ − ξ0 )2 IC (ξ) = I0 exp −8 , (1.29) w2 √ with I0 = 8/π P0 /w [92]. Here, P0 is the total light power, w is the 1/ e2 -width along the cantilever axis, and x0 is the position of the spot center on the cantilever beam, as illustrated in Fig. 1.11. The spot size w is normalized to the cantilever length. The corresponding real scalar field is (2 (ξ − ξ0 ))2 E c (ξ, ξ0 ) = I0 exp − . (1.30) w2 For small deflections Aϕ(x) λ (A is the oscillation amplitude), the modal output coupling factor is ci (ξ0 ) = Si− /A, where the difference signal Si− is obtained by integration via S− (ξ0 ) = β [0,1]
Φ(ξ) − Φ(ξ ) dξ dξ E c (ξ, ξ0 ) E c ξ , ξ0 ξ − ξ
(1.31)
[Equation (10) in [93]]. The parameter β is a prefactor that corrects for losses in the optics and also includes the wavelength of the laser. The cantilever shape Φ(ξ) is a linear combination of the orthogonal modal shapes ϕi (ξ). Thus, the modal output coupling factors can be calculated from ci (ξ0 ) = n Sig [0,1]
ϕi (ξ) − ϕi (ξ ) dξ dξ E c (ξ, ξ0 ) E c ξ , ξ0 . ξ − ξ
(1.32)
22
R.W. Stark · M. Stark
The prefactor β has been included in the normalization factor n sig . Equation (1.32) implies that the components of the output matrix C depend on both the position of the laser spot ξ0 and its spot size w. The detection optics are not changed. In static applications such as contact mode and force spectroscopy, it has been shown that maximum detection sensitivity can be obtained with a spot diameter of about w = 0.9 [92]. It is not immediately clear how it is possible to achieve a good sensitivity for the detection of higher eigenmodes. To compare the detection performance of different spot sizes, the following experimental laser alignment procedure was assumed. In the first step, the laser is adjusted to the free end of the cantilever to obtain the maximum sum signal. Then, in the second step the laser spot is moved to the free end of the cantilever until the sum signal is reduced to 90% of its maximum value. Obviously, this alignment procedure does not provide optimum sensitivity since 10% of the total laser power is lost. Nevertheless, such a procedure allows the user to adjust the laser spot to the free end without the need for high-resolution viewing optics. Bode plots of the corresponding transfer functions are illustrated in Fig. 1.12. Transfer functions G w (s) were calculated for the spot diameters w = 0.1, w = 0.3, and w = 0.9. For comparison they are normalized to the maximum static sensitivity for a spot diameter of w = 0.9 at the optimum beam alignment for quasi-static AFM measurements (ξ0 = 0.59, sum signal 99.9%). The static gains at ω = 0 were |G 0.1 | = 0.13, |G 0.3 | = 0.38, and |G 0.9 | = 0.89. This is in line with the observation that, for low frequency applications, a 1/ e2 -spot diameter of about the length of the cantilever provides the optimum sensitivity [93–95]. However, the amplitude response of G 0.3 outperformed that of G 0.9 for the eigenmodes n ≥ 3 (arrow), and G 0.1 outperformed G 0.3 for n ≤ 6 (arrow). The reason for this is that the root of ϕ3 (x) = 0 is ξ ≈ 0.7 (ϕ6 (0.9) = 0). The 1/ e2 -width of the laser spot is then of the same size as the part of the modal shape with the same slope (Fig. 1.11). Additionally, the third eigenmode is nearly canceled out in G 0.9 . Physically, this can be explained by noting that the extended laser spot integrates the slope over the illuminated area of the respective eigenmode. In the difference signal, contributions from areas with negative and positive signals cancel each other out, leading to a reduced sensitivity in this frequency range. This example shows that it is possible for higher eigenmodes to be undetectable if the laser spot is not adjusted appropriately. Thus, Fig. 1.12 illustrates the trade-off encountered during the design of the light lever detection system. A system optimized for contact mode and force spectroscopy (w ≈ 0.9) does not transmit the response of the higher eigenmodes appropriately. This can be overcome by reducing the spot diameter. The price of doing so is reduced sensitivity in the low frequency range. In a commercial AFM system, the experimentalist can usually change the position of the laser spot on the cantilever, but he cannot change its size. There are two further points that also have to be considered for the laser alignment in an existing instrument. (i) Signal artifacts can be caused by interference between the laser light reflected from the cantilever and light reflected from the sample surface. These effects are minimized by maximizing the light reflected from the cantilever (by maximizing the sum signal). This also leads to a maximized low frequency sensitivity, as required in contact mode and standard dynamic AFM. (ii) In contrast, in high frequency
1 Higher Harmonics in Dynamic Atomic Force Microscopy
23
Fig. 1.12. Bode plot of the transfer functions G w (s) for w = 0.9 (short dash), w = 0.3 (dash), and w = 0.1 (solid). The sum signal is 90% for all curves. The insets (not to scale) highlight details of the transfer functions where |G 0.1 | < |G 0.3 | < |G 0.9 |, |G 0.9 | < |G 0.1 | < |G 0.3 | and |G 0.9 | < |G 0.3 | < |G 0.1 |. Note that the third eigenmode is virtually undetectable for w = 0.9 due to an almost pole-zero cancellation (asterisk). Reprinted with permission from [96]. Copyright (2004), American Institue of Physics
experiments the laser spot should be moved to the free end of the cantilever, accepting a loss of sum signal in order to increase the high frequency sensitivity [96]. Thus, in practice the operator must account for the trade-off between high and low frequency sensitivity. Most importantly for quantitative AFM analysis, Fig. 1.12 tells us that the transfer function of an AFM critically depends on the laser beam adjustment and the laser spot size. The gain factors of the individual modes may vary as well as the frequencies of the transmission minima. Thus, in any quantitative AFM experiment involving the detection of higher eigenmodes, the transfer characteristics of the system must be measured in order to avoid large experimental errors [97, 98].
1.3 Higher Harmonic Imaging As we have seen in the preceding sections, it is the nonlinear interaction between tip and sample that gives rise to higher harmonics. By recording the amplitudes of higher harmonics of the driving frequency, images can be obtained, enabling materials to be differentiated [23, 99, 100]. The signal-to-noise ratio can be improved by employing cantilevers with tailor-made resonance characteristics [46, 101]. Under UHV conditions it was possible to achieve higher harmonic imaging with subAngstrom resolution using a light-atom probe (carbon) on a tungsten sample in frequency modulation AFM [27]. In the following, we demonstrate higher harmonic imaging in amplitude modulation AFM, employing a secondary lock-in amplifier that demodulates the AFM signal at a multiple of the driving frequency. A commercial atomic force microscope (TopoMetrix Explorer, Veeco/TM Microscopes, Sunnyvale, CA, USA) was modified to detect the anharmonic signals. In this system, the bandwidth was limited to f c ≈ 50 kHz by the photodiode pream-
24
R.W. Stark · M. Stark
plifier. Thus, signals are damped by a factor of ten at f = 500 kHz due to the low pass characteristics of the electronic circuit. An external function generator (DS 345, Stanford Research Systems) was used to generate the AFM driving signal. The signals were demodulated by a lock-in amplifier (EG&G 5302, EG&G Inc., Princeton, NJ, USA) with a time constant of 100 µs. The lock-in amplifier output (x, y) was transformed into polar coordinates (r, φ) by dedicated converter electronics. The signal amplitude r was used for AFM feedback. A second lock-in amplifier (SR 844, Stanford Research Systems) was used to detect the higher harmonic signals (Fig. 1.13). The reference signal was generated with a second function generator of the same type. To maintain phase stability, both function generators were coupled by a 10 MHz frequency standard. This separate detection of fundamental and harmonic frequencies ensured that only higher harmonics of the AFM signal were detected, avoiding possible harmonics generation caused by signal mixing in the lock-in amplifier. In order to obtain higher order harmonics within the limited bandwidth of the photodiode preamplifier, a cantilever with a low resonant frequency was employed (silicon cantilever NSC 11, lever A, v-shaped, nominal spring constant 3.0 N/m, Mikromasch, Tallinn, Estonia). The resonant frequencies of the transverse modes were f 1 = 52.2 kHz, f 3 = 264.5 kHz, and f 5 = 417.6 kHz. The eigenfrequencies f 2 and f 4 belong to torsional vibration modes of the cantilever that do not contribute the force signal. The actual spring constant c = 3.1 N/m was determined by analysis of the thermomechanical noise of the cantilever in combination with a finite element analysis [41]. To demonstrate that higher harmonic imaging allows a clear differentiation between distinct materials, a shadow evaporation mask of a 4 nm-thick platinum carbon (Pt-C) layer on a fused silica coverslip was imaged in tapping mode AFM. The cantilever was excited at its fundamental resonance frequency of f 1 = 52.2 kHz. The amplitude of the freely vibrating tip was set to A0 = 50 nm and the setpoint was adjusted to an amplitude of 60% of the free amplitude. The topographical image and
Fig. 1.13. Experimental set-up for the detection of anharmonic signals for imaging purposes. A commercial AFM is equipped with a second lock-in amplifier for the detection of anharmonic signals. Reprinted with permission from [99]. Copyright (2003), American Institue of Physics
1 Higher Harmonics in Dynamic Atomic Force Microscopy
25
the control error (amplitude) image were acquired simultaneously together with one higher harmonic image. In order to compare the images of several harmonics, higher harmonic images were obtained consecutively. Figure 1.14 shows the topography (a), control error (b) and higher harmonics (c–e). In the higher harmonic images in Fig. 1.14c–e, the material contrast between the Pt-C film and the glass substrate is prominent. The images at 3 f 1 and 8 f 1 (c,e) show that the Pt-C layer appears darker than the glass substrate. However, compared to the harmonics in Fig. 1.14c,e, a contrast reversal was observed at 5 f 1 in Fig. 1.14d. From cross-sectional analysis, it can be seen that the signal-to-noise ratio of the higher order harmonic image at 8 f 1 was increased by an order of magnitude compared to the image at acquired at 3 f 1 . The harmonics that are close to a resonance frequency of the cantilever are enhanced, thus improving the ratio between signal and instrument noise. The fifth harmonic is close to a resonance, resulting in an increased signal amplitude compared to the third harmonic. This enhancement can be seen in the cross-sectional analysis in Fig. 1.14c–e. Although simulations based on the simplified model of the tip sample contact in (1.14) explain the signal enhancement of the various modes,
Fig.1.14.(a) Topographic (b) control error and (c-e) higher order harmonic images of a 4 nm-thick Pt-C test structure on a fused silica cover slip. The driving frequency was f = 52.2 kHz, and the detection frequencies were (c) 3 f = 156.6 kHz, (d) 5 f = 261.0 kHz, and (e) 8 f = 417.6 kHz. Reprinted with permission from [99]. Copyright (2003), American Institue of Physics
26
R.W. Stark · M. Stark
they do not reproduce the contrast inversion observed in Fig. 1.14 (data not shown, see [99]). Here, more sophisticated contact mechanical models are needed that account for details of tip–sample interactions such as adhesion, capillary condensation and viscous damping. The practical use of higher harmonic signals for qualitative characterization of the imaging forces is illustrated in Fig. 1.15. A test specimen with a 100 nm-high silicon oxide grating on a silicon substrate was imaged in tapping mode. The amplitude of the freely vibrating tip was set to A0 = 45 nm, and the amplitude setpoint was adjusted to 80% of the free amplitude. The structure of the grating was obtained in the topography (a) and control error (b) images. However, in the higher harmonic image (c), a clear contrast was apparent. This can be explained by nonlinear tip sample interactions in the imaging process, that lead to the coexistence of two distinct stable states: the so-called high- and low-amplitude states [54]. A cross-sectional analysis reveals transitions of the dynamic system from the low-amplitude state in the dark regions to the high-amplitude state in the bright regions. The sharp step in the higher harmonic image (arrow, Fig. 1.4c) was accompanied by a sharp line in the control error image (b) and a small pseudo-topographical step of about 4 nm (a). Since this step was induced by the transition from the low amplitude to the high amplitude state, it does not reflect a real variation in the topography. Thus, the higher harmonic image can be used along with the phase image to assess the reliability of topographical images. Even with the limited bandwidth of this set-up, it is possible to obtain images at higher harmonics. Since the images of higher harmonics are directly related to the tip–sample forces, they can be used as monitor signals in order to optimize imaging conditions. Basically, large amplitudes in the higher harmonics indicate large repulsive tip–sample forces, whereas small amplitudes are indicative of gentle imaging conditions. In order to obtain reliable topographic information, the variations in the higher harmonic signal should also be minimized, as this corresponds to a uniform imaging state. Thus, in conclusion, there are two main benefits from the acquisition of higher harmonic data. The higher
Fig. 1.15. Detail of a silicon test structure imaged in tapping mode (scan direction right to left). (a) Topography, (b) control error and (c) eighth harmonic. The instabilities arising from the bistable behavior of the system are difficult to see in the conventional images (a) and (b). However, in the harmonic image (c), a strong contrast is apparent, indicating both operating regimes. Reprinted with permission from [99]. Copyright (2003), American Institue of Physics
1 Higher Harmonics in Dynamic Atomic Force Microscopy
27
harmonic image is useful for optimizing the imaging conditions in tapping mode, and it enables a qualitative differentiation between dissimilar materials, as we will discuss in more detail in the following section.
1.4 Spectroscopy: Distinguishing Two Polymers 1.4.1 Overview Imaging at specific higher harmonics was discussed in the previous section. Here, in turn, we focus on the spectral broadband behavior during the scan. This example describes possible strategies for exploiting the broadband information. The sample used consists of the two polymers PMMA and PS, that have similar Young’s moduli of about 3.3 GPa [102]. The local sample composition is known from the preparation process. During imaging across the boundary between both materials, the photodiode signal was recorded along different scan-lines. Figure 1.16 shows the topography and the corresponding phase image. We will focus on basic aspects that are suited to introducing concepts associated with signal analysis of dynamic AFM. More advanced methods would undoubtedly provide even more detailed results. For the sake of clarity, however, we will restrict ourselves to straightforward analysis. The first step is to find the representative spectrum of each of the materials. In a second step we use this information for material identification, in order to verify the method. In the third step the spectra are parameterized in terms of harmonic distortion, offering a direct experimental implementation.
Fig.1.16.Polymer mixture. (a) Topography and (b) phase image of the boundary region of PMMA (left) and PS (right). A significant step of approximately 40 nm separates the two polymers, as is apparent in the topography. PS appears brighter in the phase image. One scan-line is highlighted (see text). Note the groove structure traversing the PMMA in the lower half of the images. Scales (black to white): 62 nm (topography), 30◦ (phase). The scale bar equals 500 nm
28
R.W. Stark · M. Stark
1.4.2 Experimental Details The sample (courtesy of H. Sturm, BAM, Braunschweig, Germany) was prepared by dropping melts of poly(methylmethacrylate) (PMMA) poly-(methylmethacrylate), i.e. PMMA and poly(styrol) (PS) onto a freshly cleaved salt crystal. The structure was embedded in epoxy resin. After dissolving the salt, the fairly smooth structure shown in Fig. 1.16 is left. During the preparation process, the sample was precharacterized to clearly locate the domains of PMMA and PS. Imaging was carried out on a commercial AFM (Nanoscope IIIa, Digital Instruments, Santa Barbara, CA, USA) with purpose-built electronics for the extraction of the photodiode signal. A high-pass filter was used to eliminate drift in the photodiode signal. After filtering and pre-amplification (SR560, Stanford Research Systems, Sunnyvale, CA), the signal was recorded at 5 M sample/s, at 12 bit resolution (DACQ-board PCI-6110 E controlled by LabView software, both National Instruments, Austin, TX), and analyzed off-line. The v-shaped cantilever (NSC 11, lever A, v-shaped, nominal spring constant 3.0 N/m, Mikromasch, Tallinn, Estonia) was driven at its fundamental resonance frequency of 44.3 kHz. At an imaging scan-rate of 2.03 scan lines per second and 512 pixels per line, this frequency corresponds to approximately 21.3 oscillations per pixel. The image was acquired at a 67% set-point of 100 nm free amplitude. During scanning, the conditioned photodiode signal and the topographic signal were recorded simultaneously. The data acquisition was not synchronized to the scanning, in order to capture trace, retrace and possible transients. One time-trace of 1.5 × 106 samples (300 ms of data) covers 623.6 image pixels, which is more than one scan-line. Time-traces were recorded during several images. As drift demanded a readjustment of the set-point, several curves exhibited different fundamental frequency amplitudes. These curves were rejected. The remaining six time-traces were acquired under constant conditions within two subsequent images. Five of them were used to construct an ensemble for determining the average spectra, while the sixth trace was used as an independent validation trace. 1.4.3 Signal Analysis Figure 1.17 depicts the raw data of the scan-line highlighted in Fig. 1.16. To emphasize the digital nature of the data and to emphasize the character of a time-trace we give the raw units – least significant bit (LSB) and time. A step of approximately 40 nm visible at the boundary of the two materials gives a clear landmark. The material boundary is shown in Fig. 1.17, as well as the reversal of scan-direction. Below the overview, a few oscillation periods recorded on the two materials are shown as examples of the typical signal shape. Note that the RMS-signal amplitude was used as the input for the feedback loop. Important variations in amplitude occur after the step in topography. At the step, the tip is slightly withdrawn from the sample, increasing the amplitude of the fundamental oscillation while at the same time decreasing the strength of the
1 Higher Harmonics in Dynamic Atomic Force Microscopy
29
Fig. 1.17. Raw data associated with the scan-line highlighted in Fig. 1.16: (a) topography, (b) time-trace of the detector signal, (c) examples of the signal recorded on the two materials. To stress the character of the raw data, we kept the units of “least significant bits” (LSB). The step in topography measures approximately 40 nm and separates the two polymers as indicated. While the time-trace was recorded, the scan-direction was reversed (“Trace” to “Retrace”, as indicated). As the differences between the cantilever motions on PMMA and PS cannot be identified by eye, signal analysis methods are necessary
tip–sample impact. As will be shown later, this topographically-induced transient response leaves a clear fingerprint. A visual comparison of the cantilever response on both materials (Fig. 1.17c) does not allow us to estimate signal distortion, nor to distinguish between the materials. The differences are too small, partly because of the scanning conditions, and partly because they have similar material properties. Averaging techniques are necessary to extract characteristic differences. For this purpose, two respective sub-ensembles were created from all of the acquired scan-lines containing data taken on PMMA and PS. As the material boundary is known, sorting the data is straightforward. To exclude boundary effects, data close to the material step were not considered. Furthermore, one scan line was completely excluded from the sub-ensembles and will serve as an independent data set for testing. A Fourier transformation of nonoverlapping sections of 4096 points (0.8192 ms or approximately 36.3 oscillation periods) led to ensembles of spectra containing 714 members in the case of PS and 567 members in the case of PMMA. Using iterated correlation averaging, the characteristic amplitude spectra on PMMA and PS (Fig. 1.18) were obtained from a final average of 200 spectra each. At the fundamental frequency (44.32 kHz), the magnitudes of both spectra are equal, due to feedback regulation, so the spectra were normalized to the amplitude at that frequency. Clusters of peaks at multiples of the fundamental frequency are clearly visible, as well as the modal structure imposed by the spectral response of the cantilever. The DC contribution does not contain valuable information, because the signal is high-pass filtered at 14.5 kHz. Briefly comparing the spectra, no particular feature is striking enough to separate both materials. However, a detailed comparison (Fig. 1.19) reveals important differences, which are discussed in the following.
30
R.W. Stark · M. Stark
Fig. 1.18. Characteristic amplitude spectrum of the AFM signal, as obtained on (a) PMMA and (b) PS. Both spectra are normalized to the amplitude at the first harmonic (in other words the driving frequency, which is set to the fundamental resonance of the free lever). Each spectrum represents the average of 200 raw spectra (see text)
A systematic difference between the spectra is present in the frequency group assigned to the third oscillatory eigenmode of the lever around harmonic 13. In this frequency band, the PMMA amplitude is always larger to that for PS. Figure 1.19b gives a summary of the differences between the two spectra relative to the average
An,PMMA + An,PS . At this point, one value for each harmonic, An,PMMA − An,PS important observation should be stressed. The difference between the spectra of the two materials is by no means uniform. The time-course of the interaction on the two materials varies not only in its strength but also in its shape, which points to dissipative effects. Qualitatively, the impact of the tip on the sample associated with the spectrum is faster and/or harder on PMMA compared to PS. Rather than changing the elastic behavior, we suspect differences in the viscoelastic, adhesion or wetting properties at the origin. There is also a significant contrast in the second harmonic. It is known from careful inspection of the instrument that the second harmonic is
Fig. 1.19. (a) Harmonics spectra measured on PMMA and PS. (b) Comparison of the higher harmonics measured on PMMA and PS. Positive values indicate that their is a higher relative contribution for PMMA at that frequency than for PS
1 Higher Harmonics in Dynamic Atomic Force Microscopy
31
not necessarily a good spectral indicator, as it is already present in the excitation. It might also be corrupted by nonlinearities of the detection. Are the differences in the spectra, as detailed above, really significant enough to distinguish both materials? This question is addressed using cross-correlation of the characteristic spectra with spectra along the scan-lines. We define the identification parameter ID as the ratio between the cross-correlation of the spectrum AScan-line (ω) of the scan-line with the characteristic spectrum APMMA (ω) of PMMA and the crosscorrelation of the spectrum of the scan-line with the characteristic spectrum APS (ω) of PS. Both cross-correlations around time t are only evaluated on the frequency band of the third eigenmode of the lever. Thus: APMMA (ω) × AScan-line (ω) − 1 (1.33) ID(t) = APS (ω) × AScan-line (ω) ω ∈ Band of third eigenmode For ID (t) < 0, the material around time t on the time-trace is identified as PS, for ID (t) > 0 the material is identified as PMMA. We first apply this test to the marked scan-line (Fig. 1.17). Figure 1.20 shows the smoothed identification parameter ID(t) along the scan-line together with the raw-data of the topography signal. The inset recalls the topographic image. Indeed, the topographic step marks the material boundary, which is again found by the identification parameter. Remarkably, a dip in the topographic scan-line at around 20 ms is identified as PS (marked by arrows). This position matches a pronounced groove in the topographic image (arrow). From the identification parameter ID(t), as well as from careful inspection of the topographic and phase images, we assume the groove to be a fracture penetrating the covering layer of PMMA into the underlying PS. Previously, the spectral details were used to analyze the time traces. Now, in fact, we conceive the scan line as a variation of a quantity with the position on the sample. Again we focus on the scan-line highlighted in Fig. 1.16. The topography, the
Fig.1.20.Material identification for the highlighted scan-line (inset: topographic image) using the identification parameter defined in (1.33). The topography along the scan-line is given together with the identification parameter ID. The material in the groove (arrows) is identified as PS (see text)
R.W. Stark · M. Stark
32
relative phase lag, and the harmonic signal distortion are all considered, as illustrated in Fig. 1.21. For the phase lag, the average of all lines in the image is also given (thick line). Fast variations linked to features in the topography are smoothed out, and thus the average scan line is representative of the phase difference on the two materials. In the definition of the phase, we use positive values for a signal delayed with respect to the average signal, and vice versa for negative values. Thus, the more positive the phase lag, the higher the dissipation. Regarding the scan-line, we state a phase difference of 1.5◦ , indicating a higher dissipation on PS. A calculation of the total harmonic signal distortion according to A2 (nω0 ) n=2,3... THD = A2 (nω0 ) n=1,2,3...
yields an overall measure of the signal content in higher harmonics. For the case presented, this overall quantity distilled from the full spectrum does not show a significant difference for the two materials. The THD remains at about 5%, and only drops at the topographical step, which is the clear fingerprint of the control error. By defining a modal harmonic distortion where the distortion is only evaluated in a frequency band around a distinct eigenmode of the lever, we have found a material-sensitive parameterization. Figure 1.21d shows the modal harmonic distortion evaluated for the third flexural eigenmode of the lever (including harmonics 9–17). The modal harmonic distortion in the high-frequency band is more pronounced on PMMA than on PS. This example shows how to define a suitable parameterization that may provide a material specificity that is similar to that yielded by the approach using the characteristic spectra. However, the full spectra enables a verification of whether the chosen parameterization is sharp enough to separate materials or material properties in the intended way.
Fig. 1.21. (a) Topography, (b) phase, (c) total and (d) modal harmonic distortion. Both materials can be distinguished in the phase signal and in the modal harmonic distortion. The total harmonic distortion does not provide a sufficient contrast
1 Higher Harmonics in Dynamic Atomic Force Microscopy
33
1.5 Outlook This chapter has demonstrated that a deeper understanding of the cantilever dynamics permits subtle experiments probing surface forces that can be used to discriminate dissimilar materials. The relation between higher harmonics and different sample properties such as viscoelasticity, adhesion, wetting properties, surface potential, polarizability (van der Waals interaction) or specific chemical properties is not yet completely understood. However, there are several lines of development based on a full spectral analysis of the AFM signal that will provide deeper insights into short-range surface forces in the future. In order to correlate the cantilever dynamics with surface properties, a reconstruction of the forces acting at the tip over time can provide further information. Although a similar inverse problem for the simpler case of a periodically-forced harmonic oscillator was solved more than a century ago [103], a full spectral inversion is difficult due to the limited signal-to-noise-ratio encountered in AFM measurements [104, 105]. However, by taking advantage of the periodicity of the tip motion in dynamic AFM, it is possible to reconstruct the tip–sample forces [76]. Progress in the determination of surface forces can also be expected from analyzing the system’s response to a parametric excitation. By driving the cantilever at a subharmonic of a mechanical resonance, small signals can be enhanced, permitting identification of materials [106, 107]. Feedback schemes based on the detection of higher harmonics will further enhance the performance and force sensitivity of AFM measurements [27, 51, 89]. The quantification of surface forces demands a comprehensive theory of the dynamics of AFM which must cover (among others) the full range of AFM techniques, from contact mode to ultrasonic AFM and tapping mode to noncontact AFM. We did not, however, aim to solve this task by discussing the generation of higher harmonics in atomic force microscopy. Rather, we restricted ourselves to aspects of the AFM dynamics, where the motion remains periodic. Still, we hope that the concepts on which we base our considerations may help to advance the theoretical understanding of dynamic AFM. Acknowledgements. We are indebted to Wolfgang Heckl (LMU Munich, Germany), Andreas Stemmer (ETH Zurich, Switzerland), Reinhard Guckenberger and Fritz Keilmann (both MPI for Biochemistry, Martinsried, Germany), who gave us the opportunity to pursue our investigations and provided valuable discussions. Without the many fruitful discussions with Georg Schitter (UCSB, USA) and Reiner Hillenbrand (MPI for Biochemistry, Martinsried, Germany), much of the work discussed here would not have been possible. RWS gratefully acknowledges financial support from the German Federal Ministry for Education and Research (BMBF) within the programme “Young Scientists Competition Nanotechnology” (Grant 03N8706) and the Swiss Commission for Technology and Innovation (KTI, TopNano21, Grant 6351.1).
R.W. Stark · M. Stark
34
References 1. 2. 3. 4. 5. 6. 7. 8. 9. 10. 11. 12. 13. 14. 15. 16. 17. 18. 19. 20. 21. 22. 23. 24. 25. 26. 27. 28. 29. 30. 31. 32. 33. 34. 35. 36. 37. 38. 39. 40. 41. 42. 43. 44. 45.
Zhong Q, Inniss D, Kjoller K, Elings VB (1993) Surf Sci 290:L688 Magonov SN, Elings V, Whangbo MH (1997) Surf Sci 375:L385 Noy A, Sanders CH, Vezenov DV, Wong SS, Lieber CM (1998) Langmuir 14:1508 Cleveland JP, Anczykowski B, Schmid AE, Elings VB (1998) Appl Phys Lett 72:2613 Magonov SN (2003) In: Bhushan B, Fuchs H, Hosaka S (eds) Applied scanning probe methods. Springer, Berlin Heidelberg New York, p 207 Stark M, Möller C, Müller DJ, Guckenberger R (2001) Biophys J 80:3009 Dürig U, Gimzewski JK, Pohl DW (1986) Phys Rev Lett 57:2403 Fain SC, Barry KA, Bush MG, Pittenger B, Louie RN (2000) Appl Phys Lett 76:930 Stark RW (2004) Nanotechnology 15:347 Su C, Huang L, Kjoller K (2004) Ultramicroscopy 100:233 Schirmeisen A, Anczykowski B, Fuchs H (2003) In: Bhushan B, Fuchs H, Hosaka S (eds) Applied scanning probe methods. Springer, Berlin Heidelberg New York, p 3 Whiston GS (1987) J Sound Vib 118:395 Hunt JP, Sarid D (1998) Appl Phys Lett 72:2969 Salapaka S, Dahleh M, Mezic I (2001) Nonlinear Dynam 24:333 Wen G, JianHua-Xie, Daolin-Xu (2004) J Appl Mech–T ASME 71:579 Burnham NA, Behrend OP, Ouvelvey F, Gremaud G, Gallo PJ, Gourdon D, Dupas E, Kulik AJ, Pollock HM, Briggs GAD (1997) Nanotechnology 8:67 Nony L, Boisgard R, Aimé JP (1999) J Chem Phys 111:1615 Lee SI, Howel SW, Raman A, Reifenberger R (2002) Phys Rev B 66:115409 Salapaka MV, Chen DJ, Cleveland JP (2000) Phys Rev B 61:1106 Dürig U (1999) Appl Phys Lett 75:433 Stark RW, Heckl WM (2000) Surf Sci 457:219 Dürig U (2000) New J Phys 2:5 Hillenbrand R, Stark M, Guckenberger R (2000) Appl Phys Lett 76:3478 Stark M, Stark RW, Heckl WM, Guckenberger R (2000) Appl Phys Lett 77:3293 Sahin O, Atalar A (2001) Appl Phys Lett 79:4455 Balantekin A, Atalar A (2003) Phys Rev B 67:193404 Hembacher S, Giessibl FJ, Mannhart J (2004) Science 305:380 Tamayo J, Humphris ADL, Owen RJ, Miles MJ (2001) Biophys J 81:526 Sebastian A, Salapaka MV, Chen DJ, Cleveland JP (1999) Proc American Control Conf (ACC), 2–4 June 1999, San Diego, CA, USA, 1:232 Sebastian A, Salapaka MV, Chen DJ, Cleveland JP (2001) J Appl Phys 89:6473 Wei B, Turner JA (2001) AIP Conf Proc 557B:1658 Hu SQ, Howell S, Raman A, Reifenberger R, Franchek M (2004) J Vib Acoust 126:343 Butt HJ, Jaschke M (1995) Nanotechnology 6:1 Rabe U, Janser K, Arnold W (1996) Rev Sci Instrum 67:3281 Salapaka MV, Bergh HS, Lai J, Majumdar A, McFarland E (1997) J Appl Phys 81:2480 Zypman FR, Eppell SJ (1998) J Vac Sci Technol B 16:2099 Stark RW, Drobek T, Heckl WM (1999) Appl Phys Lett 74:3296 Drobek T, Stark RW, Gräber M, Heckl WM (1999) New J Phys 1:15.1 Scherer V, Arnold W, Bhushan B (1999) Surf Interf Anal 27:578 Drobek T, Stark RW, Heckl WM (2001) Phys Rev B 64:045401/1 Stark RW, Drobek T, Heckl WM (2001) Ultramicroscopy 86:207 Reinstaedtler M, Rabe U, Scherer V, Turner JA, Arnold W (2003) Surf Sci 532-535:1152 Kikukawa A, Hosaka S, Imura R (1996) Rev Sci Instrum 67:1463 Glatzel T, Sadewasser S, Lux-Steiner MC (2003) Appl Surf Sci 210:84 Rodríguez TR, García R (2004) Appl Phys Lett 84:449
1 Higher Harmonics in Dynamic Atomic Force Microscopy
35
46. Sahin O, Yaralioglu G, Grow R, Zappe SF, Atalar A, Quate C, Solgaard O (2004) Sensor Actuat A 114:183 47. Mackel R, Baumgartner H, Ren J (1993) Rev Sci Instrum 64:694 48. Kikukawa A, Hosaka S, Imura R (1995) Appl Phys Lett 66:3510 49. Nonnenmacher M, O’Boyle MP, Wickramasinghe HK (1991) Appl Phys Lett 58:2921 50. Jacobs HO, Knapp HF, Muller S, Stemmer A (1997) Ultramicroscopy 69:39 51. Okamoto K, Sugawara Y, Morita S (2002) Appl Surf Sci 188:381 52. van Noort SJT, Willemsen OH, van der Werf KO, de Grooth BG, Greve J (1999) Langmuir 15:7101 53. Gleyzes P, Kuo PK, Boccara AC (1991) Appl Phys Lett 58:2989 54. García R, San Paulo A (2000) Phys Rev B 61:R13381 55. Behrend OP, Oulevey F, Gourdon D, Dupas E, Kulik AJ, Gremaud G, Burnham NA (1998) Appl Phys A 66:S219 56. Rodríguez TR, García R (2002) Appl Phys Lett 80:1646 57. Kolosov OV, Castell MR, Marsh CD, Brix A (1998) Phys Rev Lett 81:1046 58. Hirsekorn S (1998) Appl Phys A 66:1 59. Yaralioglu GG, Atalar A (1999) Rev Sci Instrum 70:2379 60. Arinero R, Leveque G (2003) Rev Sci Instrum 74:104 61. Chudoba T, Schwarzer N, Richter F (1999) Thin Solid Films 355–356:284 62. Turner JA, Hirsekorn S, Rabe U, Arnold W (1997) J Appl Phys 82:966 63. Clark RL (1997) J Dyn Syst–T ASME 119:390 64. Reza Moheimani SO (2000) J Dyn Syst–T ASME 122:237 65. Hatch MR (2001) Vibration simulation using MATLAB and ANSYS. Chapman & Hall/CRC, Boca Raton, FL 66. Argyris J, Mlejnek H-P (1988) Die Methode der finiten Elemente. Vieweg, Braunschweig/Wiesbaden 67. Clough RW, Penzien J (1993) Dynamics of structures. McGraw-Hill, Singapore 68. Rinaldi G, Packirisamy M, Stiharu I (2004) Int J Nanotechnol 1:292 69. Spector VA, Flashner H (1990) J Dyn Syst–T ASME 112: 186 70. Derjaguin BV, Muller VM, Toporov Yu P (1975) J Colloid Interf Sci 53:314 71. Gannepalli A, Mallapragada SK (2001) Nanotechnology 12:250 72. Haefliger D, Plitzko JM, Hillenbrand R (2004) Appl Phys Lett 85:4466 73. Boyer L, Houze F, Tonck A, Loubet JL, Georges JM (1994) J Phys D Appl Phys 27: 1504 74. Hao HW, Baro AM, Saenz JJ (1991) J Vac Sci Technol B 9(2):1323 75. Dianoux R, Martins F, Marchi F, Alandi C, Comin F, Chevrier J (2003) Phys Rev B 68:45403 76. Stark M, Stark RW, Heckl WM, Guckenberger R (2002) Proc Natl Acad Sci USA 99:8473 77. Stark RW, Schitter G, Stark M, Guckenberger R, Stemmer A (2004) Phys Rev B 69:085412 78. Sader JE (1998) J Appl Phys 84:64 79. Fleming AJ, Reza Moheimani SO (2003) IEEE T Contr Syst T 11:726 80. Miu DK (1993) Mechatronics. Springer, Berlin Heidelberg New York 81. Yuan K, Liu LY (2003) J Robotic Syst 20:581 82. Hölscher H (2002) Surf Sci 515:517 83. Rodríguez TR, García R (2003) Appl Phys Lett 28:4821 84. Hao HO, Baró AM, Saenz JJ (1991) J Vac Sci Technol B 9:1323 85. Stark RW (2003) Proc 1st Int Meeting on Applied Physics 2003 (aphys2003), 13–18 October 2003, Badajoz, Spain, arXiv:physics/0501061 86. Sasaki N, Tsukada M, Tamura M, Tamura R, Abe K, Sato N (1998) Appl Phys A 66:S287 87. Basso M, Giarré L, Dahleh M, Mezic I (2000) J Dyn Syst–T ASME 122:240 88. Rützel S, Lee SI, Raman A (2003) Proc R Soc Lond A 459:1925 89. Schiener J, Witt S, Stark M, Guckenberger R (2004) Rev Sci Instrum 75:2564
36
R.W. Stark · M. Stark
90. Proksch R, Schäffer TE, Cleveland JP, Callahan RC, Viani MB (2004) Nanotechnology 15:1344 91. Schäffer TE, Fuchs H (2005) J Appl Phys 97:083524 92. Schäffer TE (2002) J Appl Phys 91:4739 93. Schäffer TE, Hansma PK (1998) J Appl Phys 84:4661 94. Putman CAJ, de Grooth BG, van Hulst NF, Greve J (1992) J Appl Phys 72:6 95. Gustafsson MGL, Clarke J (1994) J Appl Phys 76:172 96. Stark RW (2004) Rev Sci Instrum 75:5053 97. Scherer MP, Frank G, Gummer AW (2000) J Appl Phys 88:2912 98. Stark M, Guckenberger R, Stemmer A, Stark RW (2004) Proc IEEE Nano 2004, 17–19 August 2004, Munich, Germany 99. Stark RW, Heckl WM (2003) Rev Sci Instrum 74:5111 100. Crittenden S, Raman A, Reifenberger R (2004) Workshop on Advanced Dynamic AFM Methods, 8–10 October 2004, Tres Cantos, Madrid, Spain 101. Sahin O, Quate CF, Solgaard O, Atalar A (2004) Phys Rev B 69:165416 102. Bandrup J, Immergood EH (eds) (1989) Polymer handbook. Wiley, New York 103. Franklin WS (1894) Phys Rev 1:442 104. Todd BA, Eppell SJ, Zypman FR (2001) Appl Phys Lett 79:1888 105. Todd BA, Eppell SJ (2003) J Appl Phys 94:3563 106. Patil S, Dharmadhikari CV (2003) Appl Surf Sci 217:7 107. Abdel-Rahman EM, Nayfeh AH (2005) Nanotechnology 16:199
2 Atomic Force Acoustic Microscopy Ute Rabe
Abbreviations a1 , a2 , a3 , a4 and A1 , A2 , A3 , A4 aC α A b cP dY 0 , d X0 δn , δL E E∗ ε ET , ES G∗ G T, G S Fn , FL f ϕ φ, φLat Φ γ , γLat h ηAir I L L1 L2 ∗ k∗ , kLat kC
Constants in the shape function y(x) Contact radius Wave number of the flexural waves Cross-section area of the cantilever Thickness of the cantilever Ratio φLat /φ Normalized amplitude of the sensor tip in y- and x-direction, respectively Normal, lateral contact deflection (in the coordinate system of the sample surface) Young’s modulus of the cantilever Reduced Young’s modulus of the contact Displacement of the additional mass m L from the center of the beam Young’s modulus of the tip, the surface Reduced shear modulus of the contact Shear modulus of the tip, the surface Normal, lateral forces (in the coordinate system of the sample surface) Frequency Tilt angle of the cantilever Dimensionless normal, lateral contact function Phase Normal, lateral contact damping Height of the sensor tip Damping constant describing losses by air Area moment of inertia Length of the cantilever Distance from the fixed end of the cantilever to the position of the tip Distance from the free end of the beam to the tip Normal, lateral contact stiffness Static spring constant of the cantilever
38
m∗, m mL M MT , MS N(α), N0 (α) p, pLat Q R ρ S S0 , S1 , S2 , S3 , S4 σ t u0 w x, x2 y, y2 X, T , U ω Ω ψ AFAM AFM FMM SAFM SAM SLAM SMM UAFM UFM
U. Rabe
Effective mass, real mass of the cantilever Additional mass Moment Indentation modulus of the tip, the sample surface Denominators in the formulas for forced vibration of the beam Dimensionless normal, lateral contact damping Quality factor Radius of the sensor tip Mass density of the cantilever Contact area Terms in the characteristic equation Sensitivity Time Amplitude of excitation Width of the cantilever Coordinate in length direction of the cantilever Deflection of the cantilever in its thickness direction Auxiliary functions in the boundary conditions Circular frequency Characteristic function ψ = αL dimensionless wave number Atomic force acoustic microscopy Atomic force microscopy Force modulation microscopy Scanning acoustic force microscopy Scanning acoustic microscopy Scanning local acceleration microscopy Scanning microdeformation microscopy Ultrasonic atomic force microscopy Ultrasonic force microscopy
2.1 Introduction Materials with an artificial nanostructure such as nanocrystalline metals and ceramics or matrix embedded nanowires or nanoparticles are advancing into application. Polymer blends or piezoelectric ceramics are examples for materials of high technical importance possessing a natural nanostructure which determines their macroscopic behavior. Structures such as thin films or adhesion layers are of nm dimensions in only one direction, but micromechanical devices and even nano-devices are feasible which are of nm size in three dimensions. In the nm range the mechanical properties such as hardness or elastic constants and the symmetry of the crystal lattice can vary with the size of the object. Furthermore, the properties of structures with nm-dimensions depend strongly on the surrounding material and on the boundary conditions in general. Therefore there is a need to measure mechanical properties on a nano-scale.
2 Atomic Force Acoustic Microscopy
39
2.1.1 Near-field Acoustic Microscopy Ultrasonic imaging based on transmission and reflection of ultrasonic waves has been used for a long time for elasticity measurements and flaw detection in different areas such as physics, nondestructive testing and medicine. By measuring the dispersion of laser generated surface acoustic waves in the frequency range of several 10 MHz up to several 100 MHz, the elastic constants of thin films can be determined [1]. The distance covered by the acoustic wave between the generating laser spot and the receiver (about 10 mm) defines the lateral resolution of this technique. In the classical scanning acoustic microscopy (SAM), which was developed in the 1970th, an acoustic wave is focused onto the sample surface by a sapphire lens, and the reflected acoustic waves are detected [2]. The imaging contrast depends on the acoustic impedance ρv(ρ = mass density of the sample, v = sound velocity) and consequently on the elastic constants of the sample. Defects like cracks, inclusions or mechanical stresses influence the acoustic impedance and can also be imaged if they are in a certain penetration depth inside the sample. According to Abbe’s principle, techniques using focused waves are restricted in their lateral resolution to about half a wavelength. A focused acoustic beam in water yields a spot diameter of about 1 µm at 1 GHz frequency. The local resolution can be improved if an acoustic wave is guided towards the sample by a structure which is smaller and closer to the surface than the acoustic wavelength. Different acoustic microscopes based on this near-field principle were proposed [3–6]. One drawback of this type of microscope is a low signal level because the traveling acoustic waves have to pass through an nm-scaled structure. Alternatively, the near-field sensor can be constituted by a small object which vibrates at one of its resonant frequencies. Güthner et al. used a resonating tuning fork [7] vibrating at 33 kHz in air. One corner of the tuning fork served as a sensor tip. Hydrodynamic interaction between the senor tip and the sample surface damps the vibration and shifts the resonant frequency of the tuning fork. As the damping depends mainly on the thickness of the air layer between sensor and sample, there is almost no contrast by the elasticity of the sample, but the technique can be used to image topography. More recently, tuning forks or length extension quartz resonators are used as force sensors for high-resolution atomic force microscopy in air and in vacuum [8]. After the invention of the Atomic Force Microscope (AFM) [9] near field microscopy was strongly promoted and various operation modes and related techniques emerged. Since 1993, several microscopes combining AFM with ultrasonic imaging have been developed, named for example ultrasonic force microscopy (UFM) [10], scanning acoustic force microscopy (SAFM) [11], atomic force acoustic microscopy (AFAM) [12], and ultrasonic atomic force microscopy (UAFM) [13]. These techniques can be considered as special types of dynamic force microscopy or as nearfield techniques from the point of view of ultrasonic imaging. The sensor tip of the AFM has a radius of only several nm up to several 100 nm. The tip–sample contact radius, which is orders of magnitude smaller than the acoustic wavelength, defines the local resolution. To reach high local resolution, nanoscaled probes can either be used as emitters or as detectors of ultrasound. In the latter case acoustic waves are generated with
40
U. Rabe
conventional ultrasonic transducers, and a scanning probe microscope is used to detect the acoustic wave fields at the sample surface. In atomic force microscopy the tip–sample forces are a nonlinear function of tip–sample distance. The nonlinear forces cause frequency mixing, if an ultrasonic excitation signal is applied to a transducer below the sample and another vibration with a slightly different frequency is excited in the cantilever and its sensor tip [11, 14]. In the scanning acoustic force microscopy [14] mixing of two surface waves which propagate in different direction is exploited to image surface acoustic wave fields with submicron lateral resolution. Interference phenomena caused by scattering of a plane wave by a disk-shaped structure were observed in this way [15]. The nonlinearity of the tip–sample forces has a rectifying effect which is exploited in ultrasonic force microscopy [10, 16]. In UFM, an ultrasonic transducer generating longitudinal waves is placed below the sample. The amplitude of the sinusoidal excitation applied to the transducer is modulated with a saw-tooth signal. The acoustic wave causes a high frequency out-of-plane surface vibration with a low-frequency amplitude modulation. The sensor tip of the AFM is in contact with the vibrating sample surface and when the threshold amplitude is reached, the sensor tip lifts off from the surface. A lock-in amplifier which operates at the modulation frequency detects the envelope of the high frequency signal. This rectifying property was called “mechanical diode effect”. A qualitative image of elastic sample properties and contrast from subsurface objects can be obtained [16–18]. A rectifying effect due to the nonlinear forces is also observed when the amplitude modulated vibration is excited at the fixed end of the cantilever (“waveguide UFM”) [19]. The contrast in UFM was examined by different research groups [20, 21]. The advantage of the mixing technique and the UFM is the low bandwidth which is required for the position detector in the AFM. Because the modulation frequency can be chosen in the kHz range, a direct detection of signals at MHz or even GHz frequencies is not necessary. As both, elasticity and adhesion, contribute to the image contrast [22], it is difficult to separate surface elasticity quantitatively from adhesion. 2.1.2 Scanning Probe Techniques and Nanoindentation Different dynamic operation modes of the scanning force microscope were suggested to measure elasticity on an nm scale. In the force-modulation mode (FMM) the sensor tip is in contact with the probed surface, and the surface is vibrated normally or laterally at a frequency below the first resonance of the cantilever [23]. The amplitude or phase of the vibration of the cantilever is evaluated. Force modulation microscopy provides elasticity contrast of softer samples like for example polymers. If stiffer materials like metals and ceramics are to be examined, the contact stiffness between tip and surface becomes much higher than the spring constant of the cantilever (0.1 N/m up to several 10 N/m, depending on the type of beam) and the contrast decreases. Instead of applying the force indirectly by varying the distance between the surface and the fixed end of the cantilever, other research groups applied a magnetic force directly to the cantilever [24,25]. Some authors extend force-modulation microscopy to the higher modes of the cantilever [25–27]. Here, this type of operation is called contact-resonance spectroscopy and will be treated in detail in the next paragraphs.
2 Atomic Force Acoustic Microscopy
41
In the pulsed force mode [28] the distance between the fixed end of the sensor and the sample surface is also modulated at a frequency below the resonant frequencies of the sensor. The amplitude is so high (10–500 nm) that the tip loses contact with the sample surface during its vibration cycle. Characteristic points in the vibration signal of the cantilever are evaluated to image elasticity and adhesion. In scanning local acceleration microscopy (SLAM) the sensor tip is in contact with a sample surface that is vibrated out-of-plane with a frequency slightly above the first flexural resonance of the cantilever [29]. Using a temperature controlled SLAM instrument, Oulevey et al. observed martensitic phase transformation in NiTi-alloy [30]. Force-modulation microscopy can be considered as direct detection of low frequency acoustical vibrations by an AFM. A sensor tip which touches the sample surface during its vibration cycle for example in FMM or tapping mode [31] radiates sound into the sample, but the amplitudes are usually below the detection limit of commercial transducers [32]. If the sensor of the AFM is magnified by only one or two orders of magnitude like in scanning microdeformation microscopy (SMM), the acoustical amplitudes transmitted through the sample become detectable [33]. Subsurface features were imaged by SMM in transmission mode [34]. The vibration of the cantilever was measured with a piezoelectric element [35] or with an optical interferometer pointing onto the cantilever [36]. The AFM sensor and the SMM cantilever are so similar to each other that many aspects of the equation of motion and the contact mechanics models are identical. As the radius of the SMM sensor tip is larger than the radius of an AFM tip the tip–sample interaction is easier to control and macroscopic contact models are easier to apply. Because the contact area scales with the size of the sensor tip, the lateral resolution is lower in SMM than in the AFM based techniques. Nanoindentation, which was originally developed to measure hardness, can also be used for elasticity measurements [37]. In dynamic nanoindentation a low amplitude sinusoidal force modulation is superimposed to the quasi static load applied to the indenter. Amplitude and phase of the vibration of the electromechanical system, constituted by the indenter and the force detection unit, are evaluated to measure contact stiffness as a function of load [38]. The indenter tips are of Berkovich type made of diamond or spherical with a radius of 100 µm. The local resolution of the nanoindenter is typically 100 nm to 200 nm because of the mechanical stress field in the sample at a minimum penetration depth of about 20 nm. Seyed Asif et al. imaged the real and imaginary parts of the Young’s modulus of carbon fibers in epoxy matrix by dynamic nanoindentation [39]. Especially for examination of softer materials like polymers, dynamic nanoindentation became very popular during the last years. An overview of commercial instruments can be found for example in a publication by Bushan and Li [40]. 2.1.3 Vibration Modes of AFM Cantilevers The typical dimensions of cantilevers for atomic force microscopy are several 100 µm in length, several 10 µm in width and several 100 nm up to several µm in thickness. The sensors are small plates or beams having distributed mass, and they can be excited to different modes of vibration such as flexural or torsional modes. While
42
U. Rabe
most of the dynamic scanning probe applications relied on the fundamental modes of the beams, for noise analysis the importance of the higher eigenmodes was recognized by different authors [41, 42]. In atomic force acoustic microscopy and ultrasonic atomic force microscopy the flexural resonant frequencies of atomic force microscope cantilevers are measured [13, 43, 44]. The sensor of the AFM can be considered as a cantilever beam which is clamped at one end and free at the other end. If the sensor tip is in contact with a sample surface tip–sample interaction forces change the end conditions and all resonant frequencies of the cantilever are shifted. Furthermore, tip–sample interaction causes damping and changes the width of the resonance curves. When the cantilever is in flexural vibration, a large component of the amplitude of the tip apex is normal to the sample surface. Therefore flexural modes are used to measure normal tip–sample contact stiffness, which in turn depends on the Young’s modulus of tip and sample, on the shear modulus of tip and sample, on the contact area, and on the adhesion forces. In most cases, the flexural modes cause an angular oscillation of the cantilever beam at the position where the tip is fixed, which in turn leads to an oscillation of the tip apex parallel to the surface. This means that the flexural modes are also influenced by lateral tip–sample contact stiffness and friction. Torsion of AFM cantilevers is used to measure lateral forces and friction [45,46] and a variety of dynamic operation modes exploiting torsional vibration is known. Similar to AFAM and UAFM the torsional resonant frequency and the width of the resonant peaks can be determined to measure in-plane surface properties [47,48]. At low amplitudes the sensor tip sticks to the sample surface, and at higher amplitudes sliding sets in. The stick-slip events cause a characteristic plateau in the shape of the contact-resonance curves [49]. Torsional modes are not the only type of vibration exhibiting a strong component of lateral tip–sample amplitude. Bending of the cantilever in its thickness direction leads to non-negligible lateral tip–sample displacement [50], and lateral bending modes of the cantilever can be used for imaging and spectroscopy [51]. In the so-called “overtone atomic force microscopy” Drobeck et al. exploited the torsional vibration modes of V -shaped cantilevers to measure in-plane surface stiffness [52, 53]. Elasticity contrast was obtained on Al−Ni−Fe quasicrystal samples [52], and the lateral stiffness of Si, Al, and CdTe surfaces was evaluated quantitatively [53]. The results were obtained in ambient conditions by analysis of the thermal noise of the cantilevers.
2.2 Linear Contact-resonance Spectroscopy Using Flexural Modes Contact-resonance spectroscopy techniques which exploit the flexural modes of the cantilevers can be organized according to the method of excitation. In the AFAMtechnique a transducer below the sample excites longitudinal waves which cause outof-plane vibrations of the investigated surface (transducer 1 in Fig. 2.1) [43, 44]. Via the tip–sample contact forces the vibrations are transmitted into the cantilever. The flexural vibrations can also be excited by a transducer which generates oscillations of the fixed end of the beam (transducer 2 in Fig. 2.1). This technique (UAFM) was first
2 Atomic Force Acoustic Microscopy
43
Fig. 2.1. In the AFAM-mode the flexural vibrations of the cantilever are excited by a transducer below the sample (transducer 1). The vibrations can also be excited by a transducer which excites the fixed end of the cantilever (transducer 2, UAFM-mode). The low frequency components of the beam deflection signal are used to control the static deflection of the cantilever. The high frequency components of the signal are evaluated for example by a lock-in-amplifier for ultrasonic spectroscopy or imaging
published by Yamanaka and Nakano and continuously developed afterwards [13,54– 56]. Alternatively, a ZnO transducer can be fabricated directly on the sensor beam to excite the vibrations in the UAFM-mode [57–59]. Dupas et al. fixed one end of the cantilever to a piezoelectric bimorph [60]. For simplicity the technique is designated here by AFAM or UAFM, when the vibrations are excited by the sample surface or by the fixed end of the beam, respectively. Excitation by a concentrated harmonic force acting directly on the cantilever [25] or spectral analysis of thermomechanical noise of the sensor [52, 53] is also reported for contact-resonance spectroscopy. In the first AFAM experiments the ultrasonic transducer below the sample was excited with electrical spikes [61]. The resulting out-of-plane deflection of the investigated surface is a short pulse with a spectrum depending on the resonant frequency of the transducer and the transmission of the sample. The pulse at the surface excites a vibration in the cantilever which decays according to the time constants of contact damping and air damping. Fourier transformation of the cantilever vibrations showed that the spectrum contained contact resonances. However, with the pulse excitation the senor tip loses contact with the sample surface very easily and the signals are strongly influenced by adhesion. The current state of the art in AFAM and UAFM is to excite the vibration with sinusoidal signals and to sweep the frequency to measure spectra. Frequency sweeps are also common in other dynamic AFM operation modes, but in the techniques discussed here the sensor tip is in contact with the
44
U. Rabe
sample surface while the spectra are measured. This means that the static deflection of the cantilever must be controlled or monitored during the sweep. Furthermore, the techniques discussed here do not only use the fundamental resonant frequency of the cantilever but consider the higher modes, too. The necessary bandwidth of excitation and detection depends on the type of sensor beam which is used. Softer samples like polymers can be examined with sensors having a spring constant of only a few N/m or less, while stiffer samples require stiffer beams with several 10 N/m spring constant. As will be shown in the following, for example the first contact-resonance frequency of the types of beams listed in Table 2.2 is always lower than 1 MHz. This means that ultrasonic imaging is possible with a bandwidth of 1 MHz. For quantitative evaluation, the bandwidth should be large enough to cover two contact resonances at a minimum. The continuous wave signals are excited by a function generator. A fast lockin amplifier can be used to determine amplitude and phase of the vibration of the cantilever. Alternatively, the ultrasonic signal and reference can be down converted to a lower frequency and reference (20 kHz) and subsequently fed to a lock-inamplifier [62]. In this case the lock-in-amplifier works at a fixed lower frequency and needs not to follow the swept frequency. A network analyzer can also be used to excite and to detect the signals in spectral measurements [57]. Dupas et al. used a stroboscopic technique and increased the bandwidth of detection to 4 MHz by modulating the light intensity of the laser diode of the beam-deflection detector [60]. There are different possibilities of acoustical imaging using contact resonances which are discussed in Chap. 6. 2.2.1 Flexural Vibrations of Clamped-free Beams The most widespread commercial cantilevers are either of triangular or of approximately rectangular shape. The vibrational modes for example of V-shaped beams or dagger-shaped beams can be calculated numerically [63, 64] or using analytical approximations [65]. However, analytical formulas can be evaluated extremely fast and they may provide a deeper understanding of how the different parameters influence the vibration. This analysis will therefore be restricted to cantilevers with approximately rectangular shape because they can be described with satisfactory precision by analytical models. Under the precondition that its length is much larger than its width and thickness, the micro fabricated sensor beam can be regarded as an elastic beam. If x is the coordinate in length direction of the beam and y the coordinate in thickness direction, the equation of motion for damped flexural vibrations becomes [66]: EI
∂y ∂2 y ∂4 y + ηAir ρA + ρA 2 = 0 4 ∂x ∂t ∂t
(2.1)
where E is the Young’s modulus of the cantilever, ρ is its mass density, A is the area of its cross section, I is the area moment of inertia and ηAir is a damping constant expressing the dissipation caused by the air. y(x) is the deflection at position x, ∂y/∂x is the slope of the beam at position x, E I∂ 2 y/∂x 2 is the torsional moment, and
2 Atomic Force Acoustic Microscopy
45
E I∂ 3 y/∂x 3 is the shear force. One seeks a harmonic solution in time with angular frequency ω = 2π f . The solution of the differential equation of motion may be written:
y(x, t) = y(x) · y(t) = a1 eαx + a2 e−αx + a3 eiαx + a4 e−iαx eiωt . (2.2) The mode shape y(x) can also be expressed as: y(x) = A1 (cos αx + cosh αx) + A2 (cos αx − cosh αx) + A3 (sin αx + sinh αx) + A4 (sin αx − sinh αx) ,
(2.3)
where a1 , a2 , a3 , a4 and A1 , A2 , A3 , A4 are constants. By substituting the solution (2.2) in the equation of motion (2.1) one obtains the dispersion relation for a flexural wave with complex wave number α: E Iα4 + iρAηAir ω − ρAω2 = 0 ! 4 ρA α± = ± (ω2 ∓ iηAir ω) . EI In absence of damping the dispersion equation simplifies to: " (αL)2 1 E I f = . 2π L 2 ρA
(2.4) (2.5)
(2.6)
Boundary conditions must be fulfilled if the beam is of finite length L. By substituting the boundary conditions in the general solution one obtains a characteristic equation. For a beam with one clamped end and one free end one finds in textbooks [66, 67]: cos αL cosh αL + 1 = 0
(2.7)
The roots αn L of this equation can be calculated numerically, where n = {1, 2, 3, . . . } is the mode number. Examples are listed in Table 2.1. Using the dispersion relation one obtains the resonant frequencies of the beam. The quality factor Q of the resonances is given by: Q=
ωn ωn = ∆ω ηAir
(2.8)
According to (2.8), the quality factor Q increases with the mode number. Experimentally one often observes an increase in Q for the first modes up to 1 MHz followed by a decrease at still higher frequencies [44]. This means that the damping ηAir is in fact a function of the frequency. Quality factors of the first flexural resonances of commercial sensors in air are typically between Q = 200 and Q = 900 for sensors made of single crystal silicon. With most commercial atomic force microscopes the cantilever can be excited to forced vibration when its one end is free. The fundamental mode of the clamped-free beam and the quality factor of the resonance can be measured in this way. On the
46
U. Rabe
Table 2.1. Dimensionless wave number αn L and frequency ratio f n / f 1,free for different boundary conditions of the beam: clamped-free ( f n,free ), clamped-pinned ( f n,pin ), and clamped-clamped ( f n,clamp ) n
(αn L)free
f n,free / f 1,free
(αn L)pin
f n,pin / f 1,free
(αn L)clamp
f n,clamp / f 1,free
1 2 3 4 5 6 7
1.87510 4.69409 7.85476 10.99554 14.13717 17.27876 20.42035 ≈ 2n−1 2 π
1.00 6.27 17.55 34.39 56.84 84.91 118.60
3.92660 7.06858 10.21018 13.35177 16.49336 19.63495 22.77655 ≈ 4n+1 4 π
4.39 14.21 29.65 50.70 77.37 109.65 147.55
4.73004 7.85320 10.99561 14.13717 17.27876 20.42035 23.56194 ≈ 2n+1 2 π
6.36 17.54 34.39 56.84 84.91 118.60 157.90
other hand, the constants ρ, A, E, I, and ηAir are often unknown. It is therefore better to rewrite the dispersion relations (2.5) and (2.6) in terms of measurable quantities: " ω2 ηAir ω α± L = ±α1,free L · 4 2 ∓i 2 ω1,free ω1,free " ≈ ±1.8751 · f f 1,free
4
f f 1,free
(αL)2 = 2 . α1,free L
2 ∓i
1
f
Q 1,free f 1,free
(2.9)
(2.10)
Due to the high quality factors Q of the flexural modes in air the shift of the resonant frequencies caused by air damping is negligible. Here the resonant frequencies of the clamped-free beam are sometimes called “free” resonances. In this case “free vibration” is not meant as the opposite of “forced vibration” but relates to the end condition of the beam. The theory predicts a certain ratio of the free flexural resonant frequencies regardless of the cross section and the length of the beam, for example: f 2,free (4.6941)2 = = 6.27 . f 1,free (1.8751)2
(2.11)
The first ten solutions αn L for the clamped-free beam without damping (ηAir = 0) are listed in Table 2.1. Note that the bending modes are not equidistant in frequency. According to the dispersion equation, the frequency ω is not proportional to the wave number α, but ω ∼ α2 . For the higher modes the frequency interval to the next higher mode increases with the square of the frequency. The higher bending modes are no harmonics of the fundamental frequency.
2 Atomic Force Acoustic Microscopy
47
2.2.2 The Point-mass Model It is very common in atomic force microscopy to approximate the fundamental flexural mode of the clamped-free beam by a harmonic oscillator (Fig. 2.2). The constants of a point-mass model are chosen such that the resonant frequency of the harmonic oscillator ω0 equals the first resonant frequency of the beam ω1,free : ! kC ≡ ω0 (2.12) ω1,free = m∗ The static spring constant kC of the cantilever for forces acting at x = L is: kC =
3E I Eb3 w = L3 4L 3
(2.13)
The second expression holds for rectangular beams, where w and b are the width and thickness, respectively. The effective mass m ∗ is now calculated according to m∗ =
kC 2 ω1,free
=
3ρLwb 1 ≈ m 4 (α1,free L) 4
(2.14)
Here m is the real mass of the cantilever. The motion of the beam at the free end (x = L) can now be described by the equation of motion of a point-mass m ∗ : m ∗ y(L, t) + m ∗ ηAir y(L, t) + kC y(L, t) = 0 ¨ ˙
(2.15)
Interaction between the sensor tip located at x = L and a sample surface gives rise to forces, which can be represented by a second spring with the stiffness k∗ . The second spring leads to a change of the resonant frequency of the system according to [44, 68, 69]: " ! k∗ k ∗ + kC ω= = ω 1 + (2.16) 0 m∗ kC It has been shown that the point-mass model fails to predict quantitatively correct amplitudes and resonant frequencies when the contact stiffness k∗ is of the same order of magnitude or larger than the static spring constant kC of the sensor [70]. Nevertheless, the fundamental frequency of the clamped-free beam ω0 or f 0 = ω0 /2π, the static spring constant kC , and the effective mass m ∗ are very useful to characterize a sensor.
Fig. 2.2. Optical micrograph of an AFM cantilever and point-mass model
48
U. Rabe
2.2.3 Experiments with Clamped-free Beams With respect to application it is important to examine how well real sensors correspond to the flexural beam model. It is helpful to use a calibrated optical interferometer with a bandwidth of several MHz to examine as many of the higher modes of the cantilever as possible [44, 71]. For example, Hoummady et al. examined higher flexural modes of AFM cantilevers interferometrically in order to use them for imaging [72] and Cretin and Vairac used an optical interferometer to measure the vibration of the sensor in SMM [36]. Figure 2.3 shows a set-up with a Michelson-heterodyne interferometer [73]. The chip at which the cantilever is fixed is glued to an ultrasonic transducer (shear wave transducer V155, 5 MHz center frequency, Panametrics-NDT, Waltham, MA, USA). The transducer is excited with a function generator (model 33120A, Agilent Technologies). Due to the high quality factors Q of its modes, peak-to-peak voltages of several volts are sufficient to excite vibration amplitudes of the beam of several nm or even several 10 nm. Though a longitudinal wave transducer excites flexural waves more effectively, the shear wave transducer was chosen because it excites as many types of modes as possible. Torsional resonances and lateral modes could be examined in this way, too. Depending on the dimensions and material constants of the beam, it can happen that for example a torsional mode and a flexural mode have almost the same frequency. Such a situation leads to mode coupling [71, 74] and consequently to difficulties in quantitative evaluation. The He − Ne Laser beam of the interferometer is focused onto the cantilever with a microscope objective. The resulting spot diameter is only a few µm. The cantilevers are mounted on a motor-driven x-y table to scan their surface with the help of two stepper motors.
Fig. 2.3. Set-up of the optical interferometer to measure the amplitudes of the clamped-free cantilever vibration modes. The chip of the cantilever is glued to an ultrasonic transducer which provides an excitation of vibration up to a few MHz. The laser beam of the interferometer is focused onto the cantilever to a spot size of a few µm. Step motors controlled by a computer scan the surface of the cantilever
2 Atomic Force Acoustic Microscopy
49
Knowledge of the two-dimensional mode shape helps to identify modes which appear as unknown peaks in the resonance spectrum. The interferometer signal is read with a digital oscilloscope, amplitude and phase of the vibration are obtained by fast Fourier transformation. A three dimensional visualization of such a measurement is shown in Fig. 2.4. A spectral analysis showed that the beams made of silicon single crystal behaved linearly at vibration amplitudes of a few ten nm, i.e. they vibrated only at the frequency of excitation. After measurement of the fundamental mode the higher resonant frequencies of the clamped-free beam can be predicted with the frequency ratios in Table 2.1. Usually the values calculated in this way are close enough to the experimental frequencies to detect the higher modes easily. In detail, however, there are systematic deviations from the theory which depend on the type of beam. The deviations from theory can be visualized by dividing the frequencies of the higher modes by the theoretical ratio f n,free / f 1,free and plotting them as a function of mode number. In case of perfect correspondence of the sensor with the model such a plot would provide a horizontal line. Figures 2.5a and b show the resonant frequencies of a number of silicon beams. Typical dimensions of the beams examined here are listed in Table 2.2 The absolute resonant frequencies of the beams vary because of thickness variations of the
Fig. 2.4. Bending modes of a cantilever made of single crystal silicon measured with an optical interferometer in air. The frequency of the first mode was below detection limits of the interferometer. Mode n = 10 was not detected for unknown reasons. The dimensions of the beam were 1.61 × 45 × 440 µm3 (thickness × width × length) and the static spring constant was kC = 0.094 N/m according to the manufacturer
50
U. Rabe
Fig. 2.5. (a) Resonant frequencies of the first four flexural modes of 23 cantilevers from 6 different wafers (type FM, Nanosensors). (b) Resonant frequencies of the first three flexural modes of 19 cantilevers from two different wafers (type NCL, Nanosensors). The frequencies of the higher modes were divided by the theoretical frequency ratio f n / f 0 . Modes of each individual beam are connected by a line. The same symbol and line type was used for beams from the same wafer. In case of perfect correspondence to the flexural beam model, the frequencies would be connected by horizontal lines. The strong deviations in (b) were caused by multiple peaks Table 2.2. Typical data of single crystal silicon cantilevers used here as provided by the manufacturer (Nanosensors, NanoWorld AG, Neuchatel, Switzerland). The cantilevers are of approximately rectangular shape. The cross-section of the beams is trapezoidal Type of beam
Length L [µm]
Width w [µm]
NCL FM CONT
215–235 215–235 440–460
20–45 20–35 42.5–57.5
Thickness b Spring constant Resonant frequency [kHz] [µm] kC [N/m] 6–8 2–4 1–3
21–98 0.5–9.5 0.02–0.77
146–236 45–115 6–21
silicon wafers used for manufacturing. Furthermore, for one type of beam (FM) the frequencies increase more strongly, while for another type (NCL) they increase less with the mode number than predicted by the model. These systematic deviations are caused by details which are not considered in the simple analytical model. For example the beams are made of mechanically anisotropic material, the clamping of the fixed end is not infinitely stiff and symmetric, and the cross-section of the beams is not constant. The influence of these details on the resonant frequencies can be examined theoretically by finite-element calculations [75]. For example Hurley et al. examined the deviations caused by a triangular end of the beam (dagger shape) [64]. Another practical problem which often occurs when resonant frequencies are measured in an AFM is double peaks or even multiple peaks. Mode coupling can only happen if two modes have frequencies close to each other. Therefore it is likely that most of the unwanted maxima in the spectrum are caused by maxima which are already present in the spectrum of the vibration which excites the beam. The spectrum of the forced linear vibration is a product of the vibration spectrum of the chip and the spectrum of the cantilever. The chip of the cantilever has typical dimensions of 4 × 2 × 0.5 mm3 (length × width × thickness) and is therefore a mechanical structure with numerous resonant frequencies. The exact spectrum depends on how
2 Atomic Force Acoustic Microscopy
51
the chip is clamped [75]. In the AFAM-mode ultrasonic waves transmitted through a sample generate the surface vibration, which means that in this case the spectrum of the exciting signal depends on the material, the dimensions, and the clamping of the sample.
2.3 Contact Forces as Linear Springs and Dashpots When the sensor tip is in contact with a sample surface, the tip–sample forces change the end conditions of the beam. Figure 2.6 shows the situation schematically. The tip–sample forces are a nonlinear function of the tip–sample separation and they can also be hysteretic. Here it is assumed that the vibration amplitudes are so small that the forces can be represented by a system of linear springs and dashpots. In case of bending modes one can treat the problem in only two dimensions. There are forces normal to the surface represented by the normal contact stiffness k∗ and the contact damping γ and forces lateral to the surface represented by the lateral contact ∗ stiffness kLat and a lateral contact damping γLat . For technical reasons the cantilever is tilted with respect to the surface by an angle ϕ (11◦ to 15◦ ), i.e. the coordinate system of the surface is rotated by ϕ with respect to the coordinate system of the cantilever. The normal and lateral contact stiffness can be calculated from contact mechanics models [74,76,77]. Depending on the material of which tip and surface are made, all sorts of physical forces, including magnetic and electrostatic forces, can contribute to the contact stiffness. The different force models will not be discussed in detail here, but it will be assumed that the surface preparation was such that elastic forces prevail. Though in principle all types of forces can be measured by AFAM, predominance of elasticity can be ensured by choosing high enough static loads applied by the cantilever (several 100 nN).
Fig. 2.6. The sensor tip is in contact with the sample surface. A contact area of radius aC forms between the tip and the surface and the tip senses forces lateral and normal to the sample surface which are modeled by linear springs and dashpots
52
U. Rabe
The Hertzian model describes the contact between two nonconforming elastic bodies of general anisotropy [78]. In the simplest case the bodies are mechanically isotropic, the sample is considered as flat and the sensor tip is represented by a sphere with a radius R. If a normal force Fn acts onto the sphere, a contact radius aC forms: (2.17) aC = 3 3Fn R/4E ∗ . If the adhesion forces are so small that they can be neglected, the normal force Fn is given by the static deflection of the cantilever multiplied with the spring constant of the cantilever. The sum of the indentation in the contacting bodies, δn , i.e. the amount the two bodies approach is given by: ! 9Fn2 3 δn = , (2.18) 16RE ∗2 The normal contact stiffness k∗ is: 3 k∗ = 2aC E ∗ = 6E ∗2 RFn . Here, E ∗ is the reduced Young’s modulus of the contact which is given by
1 − νS2 1 − νT2 1 = + , E∗ ES ET
(2.19)
(2.20)
where E S , E T , νS , νT , are Young’s modulus and Poisson’s ratio of the surface and the tip, respectively. After AFAM experiments, the tip shape often deviates from that of a sphere [79]. In this case the shape of the tip can be described more generally by a body of revolution. It has been shown that for axisymmetric indenters on elastically isotropic half spaces the contact stiffness k∗ , i.e. the derivative of the applied load Fn with respect to the indention depth, δn , generally obeys the equation [80]: k∗ =
dFn 2 √ ∗ =√ SE dδn π
(2.21)
Here S = π × aC2 is the contact area. Therefore the relation E ∗ = k∗ /(2aC ) ,
(2.22)
which can be derived from the Hertzian model, still holds in this more general case. These formulas are derived on the assumptions of a frictionless contact. The Hertzian model is only valid if the contact area is small compared with the dimensions of the contacting bodies and their radii of curvature [78], which means that the contact radius must be smaller than the tip radius aC R. Linear elastic theory is only valid if the mechanical stresses remain small enough. In AFM these two conditions are easily violated when a sensor tip with a radius of a few nm contacts a metallic or ceramic sample surface.
2 Atomic Force Acoustic Microscopy
53
The contact radius defines the lateral resolution in contact-resonance spectroscopy. A typical contact radius in AFM ranges from several nm up to several tens of nanometers, depending on the tip radius and the elasticity of the tip and the sample. Many polycrystalline materials like metals and ceramics, which appear mechanically homogeneous on a macroscopic scale, show a local variation in elastic constants for a scanning probe microscope because the tip senses the individual grains within the polycrystalline aggregate. Each grain represents a small single crystal. This means that imaging by AFAM can only be explained when the sample surface is no longer treated as an isotropic material. Furthermore AFM sensor tips made of single crystalline silicon are not elastically isotropic, and this holds for other tip materials as well. Mechanically anisotropic materials are described by more than two elastic constants. In the most general case of two non-conforming bodies of general shape and anisotropy, the contact area is elliptical [78]. The reduced Young’s modulus of the contact is a function of the indentation δn , contains combinations of the elastic constants of tip and sample and cannot be separated into a sum of a contribution from tip and surface like in (2.20). Vlassak and Nix examined the indentation of a rigid parabolic punch in an anisotropic surface [81]. They showed that the contact area remains spherical if a three- or fourfold rotational symmetry axis perpendicular to the boundary exists. In this case (2.19) and (2.21) remain valid if the isotropic reduced elastic modulus E/(1 − ν2 ) is replaced by an indentation modulus that is calculated numerically from single crystal elastic constants [82]. Equation (2.20) is replaced by: 1 1 1 = + E∗ MS MT
(2.23)
where MS and MT are the indentation modulus of the sample and the tip, respectively. The required symmetry holds for silicon sensor tips which are oriented in (001) crystallographic direction. Because of its fourfold symmetry the tip does not alter the rotational symmetry if it is in vertical contact with an isotropic body or with a sample which also has a fourfold rotational symmetry axis along the tip and indentation axis. Even for bodies which do not have a three- or fourfold symmetry axis (2.23) can be used as a first approximation. The error made by application of this equation depends on the anisotropy and can be estimated [83]. The tilt angle ϕ of the cantilever causes tip–sample forces tangential to the surface when the surface is moved in its normal direction. Additionally, the flexural vibrations cause an angular deflection ∂y/∂x at the sensor-tip position and consequently a lateral deflection h∂y/∂x of the sensor tip apex. Tangential forces were treated by Mindlin [78]. The lateral contact stiffness depends on the effective shear stiffness G ∗ of the contact: dFL ∗ kLat = = 8aC G ∗ (2.24) dδL 1 2 − νS 2 − νT = + (2.25) ∗ G GS GT where δL is the lateral contact deflection, and G S and G T are the shear modulus of the sample and the tip, respectively. For isotropic bodies the ratio between the ∗ normal contact stiffness k∗ and the lateral contact stiffness kLat is independent of the
54
U. Rabe
normal force Fn : ∗ 8aC G ∗ 4G ∗ kLat = = . k∗ 2aC E ∗ E∗
(2.26)
As Mazeran and Loubet pointed out [25], for E T E S ∗ 2(1 − νS ) kLat ≈ . ∗ k 2 − νS
(2.27)
Taking a range of Poisson’s ratio from 0.1 for diamond to 0.5 for rubber, the ratio ∗ /k∗ varies from 2/3 to 18/19 with an of lateral and normal contact stiffness kLat average value of 0.85 [25]. Like in the case of the normal contact stiffness, it will be necessary in future to calculate shear stiffness, taking into account the mechanical anisotropy of the contacting bodies. An important question for nondestructive testing is whether techniques like AFAM or UAFM are able to detect sub-surface features. The typical frequency f of ultrasonic excitation is 100 kHz to 10 MHz. The velocity of longitudinal acoustic waves in the solids under examination ranges typically from v = 1 mm/µs (polymers) to v = 10 mm/µs (ceramics). In this case the acoustic wavelength λ = v/ f ranges from 100 µm to 10 cm. Consequently the acoustic wavelength is larger than the scan width of the AFM and orders of magnitude larger than the contact radius. This confirms that the vibrating tip can be seen like a dynamic indenter and the penetration depth of the ultrasonic techniques is given by the decay of the mechanical stress field in the sample. According to the Hertzian contact model the decay length is several multiples of the contact radius (see Fig. 2.7). Therefore it is possible to measure the film thickness with AFAM or UAFM [57], provided the films are thin enough. Yaralioglu et al. calculated the contact stiffness of layered materials using the impedance of a mechanical radiator [58]. They examined thin films of photo resist, W, Al, and Cu on silicon single crystal. They were able to show that in the low frequency limit ( f → 0) the impedance method provides the same results for the contact stiffness k∗ as the Hertzian contact model and that this method is well suited to
Fig. 2.7. Mechanical stress field in a Hertzian contact as a function of penetration depth z into the surface. The average normal pressure pn in the contact area is given by pn = Fn /πaC2 , where Fn is the normal force and aC is the contact radius. The compressional stresses σz and σr have their maximum at the surface and the principal shear stress τ1 reaches its maximum in the sample [78]
2 Atomic Force Acoustic Microscopy
55
calculate the influence of subsurface defects on the contact stiffness [84]. Tsuji et al. observed subsurface dislocation movement in graphite with UAFM. They calculated the influence of a subsurface layer with lower Young’s modulus on the contact stiffness using finite elements [85–88]. The penetration depth of the mechanical stress field can be enhanced by increasing the contact radius, however, this causes a loss in lateral resolution. According to Fig. 2.7 the compressional stress has its maximum at the sample surface, while the shear stress reaches its maximum below the surface. Therefore techniques which exploit lateral vibrations like torsional contact-resonance spectroscopy should be very sensitive to subsurface defects.
2.4 Characteristic Equation of the Surface-coupled Beam In the linear model shown in Fig. 2.8 the forces between the sensor tip and the surface are represented by a system of springs and dashpots. The length of the cantilever from the clamped end to the free end is L. The sensor tip is located at position L 1 and L 2 = L − L 1 is the distance between the tip position and the free end. Again, one seeks a harmonic solution in time. Two sections of the cantilever with individual solutions for the mode shapes, y1 (x1 ) and y2 (x2 ), respectively, are defined. The function y1 (x1 ) describes the amplitude of the section which begins at the clamped end at x = 0 and ends at the tip position at x = L 1 . For simplicity one can use y(x) instead of y1 (x1 ), because the two functions are identical on the first section of the beam. The function y2 (x2 ) begins at the free end of the beam and ends at the tip position at x2 = L 2 . At the clamped end of the beam the deflection and the slope of
Fig. 2.8. Linear model of the cantilever when the sensor tip is in contact with a sample surface. The tip–sample interaction forces are represented by springs and dashpots. The cantilever is tilted by an angle ϕ with respect to the surface. The sensor tip of height h is located at a position L 1 on the length axis of the cantilever. The distance of the tip to the free end of the cantilever is L 2
56
U. Rabe
the beam must be zero, while at the free end of the beam the forces and moments have to be zero. The end conditions for y(x) and y2 (x2 ) are therefore: ⎧ 2 ⎧ ∂ y ⎪ ⎪ ⎨ y(x) = 0 ⎨ 2 =0 . (2.28) x = 0 : ∂y(x) y = L : ∂x3 ⎩ ⎪ ∂ y =0 ⎪ ⎩ = 0 ∂x ∂x 3 The solution (2.3) and its derivatives together with the foregoing end conditions yield A1 = A3 = 0 for y(x) and A2 = A4 = 0 for y2 (x2 ). The shape functions therefore have the form: y(x) = A2 (cos αx − cosh αx) + A4 (sin αx − sinh αx) y2 (x2 ) = A1 (cos αx2 + cosh αx2 ) + A3 (sin αx2 + sinh αx2 ) .
(2.29)
The partial solutions y(x) and y2 (x2 ) must be coupled continuously at the tip position at x = L 1 i.e. at x2 = L 2 . ⎧ ⎨ y(x) = y2 (x2 ) (2.30) x = L 1 or x2 = L 2 : ∂y(x) ∂y2 (x2 ) ⎩ =− ∂x ∂x2 The negative sign in the equation for the derivatives appears because the x2 -axis is defined in the negative direction of the x-axis. This direction was only chosen for convenience of calculation. Note that the x-axis (and the x2 -axis) of the cantilever is not parallel to the surface when the cantilever is tilted by an angle ϕ as shown in Fig. 2.8. In this text the terms “y-axis” and “x-axis” always correspond to the coordinate system of the cantilever. The moments and the forces on the sensor tip lead to further boundary conditions at the coupling position. One can first consider a simplified case where the x-axis of the cantilever is parallel to the sample surface ∗ = 0, and γ = 0). The and only forces normal to the surface are acting (ϕ = 0, kLat boundary condition for the shear forces at x = L 1 is in this case: EI
∂3 y ∂ 3 y2 ∂y(L 1 , t) . + E I 3 = k∗ y(L 1 , t) + γ 3 ∂x ∂t ∂x2
(2.31)
The solution looked for is a harmonic wave of the form y(x, t) = y(x) exp(iωt). The time derivatives can therefore be calculated and reformulated using the dispersion relation (2.6) neglecting the air damping. This leads to the boundary condition 1 ∗ ∂ 3 y ∂ 3 y2 + = · k y(L 1 , t) + γ iωy(L 1 , t) 3 3 ∂x EI ∂x2 " $ % k∗ 1 2 = y(L 1 , t) + γ iα . EI E IρA
(2.32)
A contact function φ(α) is defined, which contains contact stiffness and contact damping:
2 Atomic Force Acoustic Microscopy
φ(α) = 3
57
k∗ + i(αL 1 )2 p . kC
(2.33)
The spring constant kC of the cantilever (2.13) was used. The dimensionless damping constant p is defined as [70]: L 1γ 3γ L1 L 1 (1.875)2 γ p= √ = = . L (1.875)2 m ∗ ω0 L mω0 E IρA
(2.34)
Substituting the contact function φ(α) in (2.31), the boundary condition now becomes φ(α) ∂ 3 y ∂ 3 y2 + = 3 y(L 1 ) . 3 ∂x 3 ∂x2 L1
(2.35)
In the same way a lateral contact function φ(α)Lat is defined: φLat (α) = 3
∗ kLat + i(αL 1 )2 pLat kc
L 1 γLat pLat = √ . E IρA
(2.36)
The angle ϕ of the cantilever with relation to the surface causes cross-coupling between lateral and normal signals. Forces Fx in length-direction of the beam acting on the sensor tip give rise to a moment M = h Fx at the end of the beam. The angular deflection ∂y/∂x of the beam at the tip position causes a deflection in x-direction h∂y/∂x of the tip apex. In summary, this leads to the following boundary conditions for the forces and the moments at the tip position: ⎧ 2 ∂y(x) ∂ y(x) ∂ 2 y2 (x2 ) ⎪ ⎪ ⎪ − X(α)y(x) − = −T(α) ⎪ 2 2 ⎪ ∂x ∂x ∂x ⎨ 2 x = L 1 or x2 = L 2 : . ⎪ 3 3 ⎪ ⎪ ∂ y(x) ∂ y2 (x2 ) ∂y(x) ⎪ ⎪ + = U(α) · y(x) + X(α) ⎩ ∂x 3 ∂x ∂x23 (2.37) The auxiliary functions T , X and U are defined as follows: T(α) =
h2 h2 φ(α) sin2 ϕ + 3 φLat (α) cos2 ϕ 3 L1 L1
X(α) =
h sin ϕ · cos ϕ [φLat (α) − φ(α)] L 31
U(α) =
1 1 φ(α) cos2 ϕ + 3 φLat (α) sin2 ϕ . 3 L1 L1
(2.38)
The four boundary conditions at the coupling position are used to determine the four unknown constants in the shape functions y(x) and y2 (x2 ). The solutions of this eigenvalue problem define an infinite set of discrete wave numbers αn . After some
58
U. Rabe
pages of calculation one obtains the following characteristic equation: Ω(α) ≡ S4 + S3 T(α) + S2 X(α) + S1 U(α) + S0 T(α)U(α) − X 2 (α) = 0 (2.39) where S0 , S1 , S2 , S3 , and S4 stand for the following terms: S0 = (1 − cos αL 1 cosh αL 1 )(1 + cos αL 2 cosh αL 2 ) S1 = α [−(1 − cos αL 1 cosh αL 1 )(sin αL 2 cosh αL 2 − sinh αL 2 cos αL 2 ) + (1 + cos αL 2 cosh αL 2 )(sin αL 1 cosh αL 1 − sinh αL 1 cos αL 1 )] S2 = 2α2 [sin αL 1 sinh αL 1 (1 + cos αL 2 cosh αL 2 ) + sin αL 2 sinh αL 2 (1 − cos αL 1 cosh αL 1 )] S3 = α3 [(sin αL 1 cosh αL 1 + sinh αL 1 cos αL 1 )(1 + cos αL 2 cosh αL 2 ) − (sin αL 2 cosh αL 2 + sinh αL 2 cos αL 2 )(1 − cos αL 1 cosh αL 1 )] S4 = 2α4 (1 + cos αL cosh αL)
(2.40)
The last term in the characteristic equation (2.39) can be further simplified by substituting the definitions of the auxiliary functions: T(α)U(α) − X 2 (α) =
h2 φ(α)φLat (α) L 61
(2.41)
2.4.1 Discussion of the Characteristic Equation In order to understand the characteristic equation of the surface-coupled beam, it is helpful to consider simple cases. If for example all the spring constants and the dashpot constants are set to zero, the auxiliary functions T(α), X(α), and U(α) become zero too. This means that all terms except S4 vanish in Ω(α) and the characteristic equation reduces to (2.7) which is the equation of the clamped-free beam. As a next step one can consider only a normal spring k∗ , the lateral spring constant and the contact damping are still considered to be zero. This means that the contact function and the lateral contact function become φ(α) = 3k∗ /kC and φLat (α) = 0, respectively. If in addition the beam is not tilted (ϕ = 0), and if the tip is located at the end of the beam (L 1 = L and L 2 = 0), the auxiliary functions X(α) and T(α) vanish and U(α) simplifies to U(α) = φ(α) = 3k∗ /kC . The characteristic equation for a clamped-spring-coupled beam [13, 44] then follows:
2 Atomic Force Acoustic Microscopy
(αL)3 (1 + cos αL cosh αL) + 3
59
k∗ (sin αL cosh αL − sinh αL cos αL) = 0 kC (2.42)
Two examples of the shape function y(x) of this case are shown in Fig. 2.9. Note that (2.42) contains the characteristic equation of the clamped-free beam and the characteristic equation of the clamped-pinned beam, combined by the factor (αL)3 kC /3k∗ . The clamped-pinned case is reached when the normal contact stiffness k∗ goes to infinity. Starting from the clamped-pinned case one can now add a lateral spring which causes feedback forces proportional to the angle of the end of the beam. A lateral spring fixed to the sensor tip is equivalent to a torsional spring which is fixed directly to the end of the beam [25]. The characteristic equation of this case can be obtained by dividing (2.39) by U(α) and subsequently considering the case U(α) → ∞. From the remaining terms S1 + S0 T(α) = 0 one obtains the following characteristic equation: 3
∗ h 2 kLat (1 − cos αL cosh αL) + αL (sin αL cosh αL − sinh αL cos αL) = 0 L 2 kC (2.43)
Finally, when the lateral spring constant too goes to infinity, one obtains a cantilever which is clamped at both ends. The simplified cases of the characteristic equation discussed above are shown in Fig. 2.9. Furthermore, the shapes of the first (n = 1) and the third (n = 3) mode are shown. In the spring-coupled cases, the mode shapes change continuously with the contact stiffness, Fig. 2.9 shows one example of normal contact stiffness and one of lateral contact stiffness. Other special cases of the characteristic equation (2.39) were published in literature [44, 60, 89]. The characteristic equation for a beam with normal and lateral springs at the end at x = L was first published by Wright and Nishiguchi. [89]. The continuous change in mode shape as a function of contact stiffness is accompanied by a continuous change in resonant frequency. The lines labeled “A” in Fig. 2.10 show the resonant frequencies of the first four flexural modes as a function of normalized contact stiffness k∗ /kC for the clamped-spring-coupled beam (2.42). In this case the contact-resonance frequencies of the n’th mode are always lower than the free resonant frequency of the subsequent mode (n + 1). The gaps in the spectrum between the clamped-pinned mode and the next clamped-free mode are shown as grey areas. If the sensor tip is moved away from the end of the beam (L 2 > 0), the maximum possible frequency shift increases. The case of a relative tip position L 2 /L = 5% is shown as lines “B” in Fig. 2.10. If it happens for a mode that the distance of its last vibration node to the end of the beam becomes equal to or larger than the distance of the tip to the end, L 2 , this mode merges with the next higher mode and the situation becomes difficult to survey. As the wavelength decreases with increasing mode number, there are always higher modes for which this limit is surmounted. In the experiments it is therefore better to evaluate only modes for which the wavelength is greater than L 2 . A torsional spring at the end of the beam (lines “C” in Fig. 2.10) also increases the shift of the resonant frequencies to higher values, such that the gaps in the spectrum disappear. The approximations for large n in Table 2.1 show that
60
U. Rabe
Fig. 2.9. Characteristic equations for some selected simple cases of the cantilever in flexural vibration. The shape functions y(x) for the first flexural mode (n = 1) and the third mode (n = 3) are shown
the frequency of the (n + 1)’th clamped-free mode equals the frequency of the n’th clamped-clamped mode. In a real experiment there will always be normal and lateral forces at the same time. However, even if the lateral contact stiffness is of the same size as the normal contact stiffness, its influence on the cantilever vibration is smaller than the influence of the normal stiffness, due to the factor h 2 /L 2 which appears in the characteristic equation. The lateral forces are transformed into a moment by the lever-arm h of the sensor tip which is shorter than the cantilever length L. Typical sensor tip heights h are 5–15 µm, typical cantilever lengths L are 100–400 µm, i.e. h 2 /L 2 ranges from 0.15 to 0.0125. As a consequence, the lateral contact stiffness influences the frequency little if the normal contact stiffness k∗ is low compared to the spring constant of the cantilever kC . At higher contact stiffness k∗ the frequency shift comes closer to its upper limit, and ∗ becomes remarkable. It was first the influence of the lateral contact stiffness kLat pointed out by Mazeran and Loubet [25] that the influence of the lateral contact ∗ stiffness kLat is high when the ratio of the normal contact stiffness to the spring constant of the cantilever k∗ /kC is high. As a consequence, lateral forces may not be neglected if contact resonances are measured with soft sensor beams on stiff surfaces.
2 Atomic Force Acoustic Microscopy
61
Fig. 2.10. Shift of the normalized resonant frequencies f n / f 0 of the first four flexural modes as a function of normalized contact stiffness k∗ /kC . The lines labeled “A” show the case when only a spring normal to the sample surface is fixed to the cantilever. In case “B” the normal spring is fixed slightly away from the free end of the cantilever. In case “C” lateral tip–sample forces act additionally to the normal forces. A constant ratio between lateral and normal contact stiffness ∗ /k ∗ = 0.85) was assumed (kLat
Dupas et al. [60, 90] calculated the characteristic equation for the complete model shown in Fig. 2.8 with an additional spring at the clamped end of the cantilever. They examined the influence of the position and of the length of the sensor tip on the frequency shift of the first flexural mode. Arinero and Lévêque [26] calculated the contact vibrations of a beam with finite elements and examined the influence of the tip among other parameters. Wu et al. examined the influence of the length of the sensor tip on the frequency shift of the vibration modes [91]. 2.4.2 Influence of an Additional Mass An additional point-mass m L on the cantilever shown schematically in Fig. 2.11 causes an inertial force proportional to −ω2 m L . The influence of the mass can be found out easily if it is located at the tip position x = L 1 on the length axis of the beam [44, 92]. In this case the auxiliary function U(α) (2.38) in the boundary conditions (2.37) changes. If the center of gravity of the mass is displaced by ε from the middle plane of the beam, a moment proportional to −ε2 ω2 m L [92] has to be added in the auxiliary function T(α). The form of the characteristic equation as well as the auxiliary function X(α) remain unchanged. With the help of the dispersion relation (2.6) one obtains: ε2 m L h2 2 2 (φ(α) sin ϕ + φ (α) cos ϕ) − (αL 1 )4 Lat L 31 L 31 m 1 1 mL U(α) = 3 (φ(α) cos2 ϕ + φ Lat (α) sin2 ϕ) − 3 (αL 1 )4 L1 L1 m T(α) =
(2.44)
62
U. Rabe
Fig. 2.11. An additional point mass m L is located on the cantilever at x = L 1 . The mass is displaced by ε from the middle plane of the beam indicated by the chain dotted line
It was assumed that ρAL 1 ≈ m, where m is the mass of the cantilever. This is a good approximation if the sensor tip is located close to the end of the beam. Without lateral forces, with a tip at the end of the beam (L 2 = 0), without tilt (ϕ = 0), and without damping one obtains the characteristic equation derived by Muraoka [92]: (αL)3 [(1 + cos αL cosh αL) − Lε 2 mmL (αL)3 ∗ (sin αL cosh αL + sinh αL cos αL)] mL k 3 − = 0 (2.45) (αL)4 + kC m sin αL cosh αL − sinh αL cos αL 2 − Lε 2 mmL (αL)3 (1 − cos αL cosh αL) 2
This equation was used to calculate the frequency shift in Fig. 2.12a. With increasing additional mass the cantilever behaves more and more like a point-mass oscillator. The frequency shift of the point-mass oscillator is according to (2.16): " k∗ f = 1+ (2.46) f0 kc This behavior is shown in Fig. 2.12 as a dashed line (p1). In case of an additional mass at x = L the point-mass model predicts the following frequency shift: " ! −1 f k∗ mL = 1+ · 1+4 (2.47) f0 kc m An additional mass increases the effective mass of the beam and lowers its first free resonant frequency. The frequency shift according to the point-mass oscillator with additional mass (2.47) is labeled (p2) in Fig. 2.12. If the additional mass is high enough (m L /m = 5) there are sections of the dispersion curves of the beam which coincide with the point-mass model. If contact-resonance frequencies are measured
2 Atomic Force Acoustic Microscopy
63
Fig. 2.12. Influence of an additional mass m L on the frequency shift of the contact-resonance frequencies (a) without lateral forces ( displacement of the mass ε = 0, m L /m = 5, position of the mass L 1 /L = 1) [92], (b) with lateral forces (position L 1 /L = 0.9, ratio of lateral contact stiffness to normal contact stiffness k∗Lat /k∗ = 0.85, beam angle ϕ = 11◦ , cantilever length divided by tip height L/h = 15, mass displacement ε = 0, m L /m = 5). The dashed lines show the frequency shift of the equivalent point-mass oscillator without additional mass (p1) and with additional mass m L (p2)
and evaluated which lie on these sections, the simple point-mass formulas can be used to calculate the normalized contact stiffness k∗ /kC from the contact-resonance frequencies [92]. Muraoka observed an improved contrast when he used a cantilever with a W-particle glued onto its end for imaging in AFAM [93]. The characteristic equation with the additional mass can also be used to calculate the influence of the sensor tip on the vibration modes. For most commercial cantilevers, however, the influence of the mass of the tip is negligible. 2.4.3 Roots of the Characteristic Equation with Damping In the discussion of the characteristic equation the influence of the contact damping has not been considered so far. In a simplified case without lateral forces and tilt of the beam, the characteristic equation becomes [70]: ∗ k 3 2 (αL) (1 + cos αL cosh αL) + 3 + i(αL) p kC × (sin αL cosh αL − sinh αL cos αL) = 0 (2.48) The solutions αn L of this equation are complex numbers. The influence of the contact damping on the real part and the complex part of the wave number is shown in Fig. 2.13 [70]. The shapes of the first three modes in the case of a ratio of the normal contact stiffness to the spring constant of the cantilever k∗ /kC = 10 and without contact damping ( p = 0) are shown as insets. With increasing contact damping p mode 1 shows stiffening behavior, i.e. the frequency increases, while
64
U. Rabe
Fig. 2.13. Influence of the dimensionless contact damping p on the first three modes in the case k∗ /kC = 10. The real part (filled symbols) and the imaginary part (open symbols) of the eigenvalues αn L are plotted as a function of p
mode 2 shows softening behavior. Both modes have a maximum of the imaginary part of the wave number in the frequency interval where the real part of αn L changes strongly. Note that the horizontal scale in Fig. 2.13 is logarithmic. The stiffness of mode 2 decreases strongly, the imaginary part of αn L increases at first, then it decreases again and in this part of the curve the absolute values of the real and the imaginary parts are identical. A closer experimental and theoretical study of how the vibration modes behave as a function of interaction damping could lead to new techniques to measure tip–sample interaction damping or even internal friction at sample surfaces.
2.5 Forced Vibration Three types of excitation shown in Table 2.3 play an important role in AFM. (a) It is possible to vibrate the clamped end of the cantilever harmonically in its thickness direction with an amplitude u c (t) = u 0 eiωt (UAFM). (b) The sample surface is set into normal vibration with an amplitude u S (t) = u 0 eiωt (AFAM). (c) A concentrated harmonic force F(t) = F0 eiωt – for example a magnetic force – acts directly on the cantilever. The excitation signal is added to the boundary conditions. Afterwards the general solution and its derivatives are substituted in the boundary conditions and the constants A1 , A2 , A3 and A4 are calculated as a function of excitation frequency. Table 2.3 shows a simplified situation with only a spring and a damper at the end of the beam. The boundary conditions are in the AFAM mode, case (b): ⎧ ∂2 y ⎪ ⎪ ⎨ 2 =0 y = a0 (2.49) x = 0 : ∂y x = L : ∂x3 =0 ⎪ φ(α) ∂ y ⎪ ⎩ ∂x = 3 (y − u 0 ) ∂x 3 L
Table 2.3. Boundary conditions and solutions for the forced flexural vibration of a cantilever beam. Three techniques of excitation are treated: (a) Vibration of the clamped end of the cantilever, (b) sample surface vibration, (c) modulated concentrated force acting at x = L
2 Atomic Force Acoustic Microscopy 65
66
U. Rabe
From the first two boundary conditions one obtains A1 = A3 = 0, and with the third boundary condition the shape function becomes: y(x) = A2 (cos αx − cosh αx) + A4 (sin αx − sinh αx)
(2.50)
From the last boundary condition the constants A2 and A4 are calculated: A2 = −
u 0 φ(α) (sin αL + sinh αL) 2N(α)
A4 =
u 0 φ(α) (cos αL + cosh αL) (2.51) 2N(α)
The denominator of the two constants in the foregoing equations is the same: N(α) = (αL)3 (1 + cos αL cosh αL) + φ(α)(cosh αL sin αL − sinh αL cos αL) (2.52) The complex amplitude of vibration is obtained by substituting (2.51) and (2.52) in (2.50): y(x) =
u 0 φ(α) [−(sin αL + sinh αL)(cos αx − cosh αx) 2N(α) + (cos αL + cosh αL)(sin αx − sinh αx)]
(2.53)
The detector, for example the laser spot of an interferometer, is usually located at the end of the beam. In this case one only needs the amplitude at x = L, and (2.53) simplifies to: y(L) = u 0
sin αL cosh αL − sinh αL cos αL N(α)
(2.54)
Commercial atomic force microscopes are generally equipped with beam-deflection sensors. Their signal is proportional to the angle of the cantilever, given by the derivative of y(x). At the end of the beam at x = L the derivative is: αLu 0 sin(αL) sinh(αL) ∂y = ∂x x=L L N(α)
(2.55)
The boundary conditions and shape functions for the three mentioned cases of excitation are shown in Table 2.3. The amplitudes and slopes in (2.54) and in (2.55) are complex numbers. Real amplitude and phase Φ of the signals are calculated here using: |y(x)| =
Im[y(x)]2 + Re[y(x)]2
Φ(x) = − arctan
Im[y(x)] Re[y(x)]
(2.56)
The normalized vertical amplitude of the sensor tip dY 0 and the normalized lateral amplitude d X0 of the sensor tip are defined according to: ∂y (2.57) dY 0 = |y(L)| /u 0 d X0 = h (L) /u 0 ∂x
2 Atomic Force Acoustic Microscopy
67
The lateral amplitude is the amplitude in x-direction, parallel to the length axis of the cantilever. Note that the vertical and lateral amplitudes dY 0 and d X0 , respectively, are only normal and lateral to the sample surface if the cantilever is not tilted (ϕ = 0). Figure 2.14 shows examples of forced vibration calculated with the formulas in Table 2.3 (a) and (b). The normalized vibration amplitude dY 0 and the normalized lateral vibration amplitude d X0 are shown for three different values of normalized contact stiffness k∗ /kC . The lateral amplitude, which is proportional to the beamdeflection signal, becomes very small in the case k∗ /kC = 10 for the first mode and very high in the case k∗ /kC = 100. The maxima are marked as (1) and (2) in Fig. 2.14(c) and (d). Figure 2.15 shows the corresponding mode shapes y(x). The shape of the first mode is similar to the shape of a pinned mode in the case k∗ /kC = 100. This leads to high lateral amplitude at the end of the beam and a strong beam-deflection signal. In the case k∗ /kC = 10 the lateral deflection becomes almost zero at the end of the beam, and the first mode is hardly visible if a beamdeflection sensor is used and if the laser spot is focused to the end of the beam. The beam-deflection detector is most sensitive when the laser spot is located in one of the nodes of the vibration mode. The first mode will therefore be detectable if the
Fig. 2.14. Forced vibration of a cantilever calculated with the formulas shown in Table 2.3 for excitation at the clamped end and excitation by the sample surface. The vertical and lateral amplitudes of the sensor tip d Y 0 and d X0 , respectively, are shown for three different values of contact stiffness. In Figs. (a) and (b) the vibration was excited at the clamped end (UAFM) and in Figs. (c) and (d) the vibration was excited by sample surface vibration (AFAM). The damping constants used for the calculation were Q 1,free = 300 and γ/(m ∗ ω0 ) = 0.4
68
U. Rabe
Fig. 2.15. Shape functions y(x) of the modes corresponding to the peaks marked as (1) and (2) in Figs. 5.1 (c) and (d). The spring and the dashpot representing the contact forces are not shown here
laser spot is moved towards the middle of the beam. However, this decreases the sensitivity of the detection system to static forces and there is the risk that a position more in the middle of the beam corresponds to an antinode of one of the higher modes. All solutions in Table 2.3 have the same denominator N(α). The denominator contains the characteristic equation (here the characteristic equation of the simplified case without tilt of the cantilever and without lateral forces). In the case of low damping the zeros of the denominator are the resonant frequencies of the system, and the resonant frequencies are independent of the method of vibration excitation, as can be seen in Fig. 2.16. The measured amplitudes, however, depend strongly on the type of excitation, on the method of detection (amplitude or slope) and on the position of the detecting laser spot on the length axis of the cantilever. In the AFAM-mode one observes anti-resonances between the resonant frequencies where
Fig. 2.16. Vertical amplitude dY 0 and lateral amplitude d X0 in the UAFM and AFAM mode. The case of a normalized contact stiffness of k∗ /kC = 10 was chosen. A measurement at the end of the beam was assumed (x = L). The vertical lines show that the detected resonant frequencies are independent of the type of excitation and also independent of whether one detects the amplitude of the beam (equal to the vertical tip amplitude) or the slope of the beam (proportional to the lateral tip amplitude) if the damping is low. The constants used for the simulation were: Resonant frequency of the clamped-free beam f 1,free = 150 kHz, Q 1,free = 300, contact damping γ/(m ∗ ω0 ) = 0.4
2 Atomic Force Acoustic Microscopy
69
Fig. 2.17. Amplitude (dashed line) and phase (continuous line) in the AFAM-mode (a) and in the UAFM-mode (b). In the AFAM-mode (a) anti-resonances accompanied by a phase shift of −π are observed. The data for the calculation were the same as in Fig. 2.16
Fig. 2.18. Forced vibration in the AFAM-mode. The lateral amplitude d X0 is shown. This signal is proportional to the beam-deflection signal. (a) Influence of the position of the sensor tip (b), influence of the lateral forces in the case of normalized contact stiffness k∗ /kC = 100, contact damping γ/(m ∗ ω0 ) = 0.4. (c) Influence of the position of the laser spot on the detected signal, (d) influence of the lateral forces in the case k∗ /kC = 1000, γ/(m ∗ ω0 ) = 2. For the lateral forces in (b) and (d) a ratio of lateral to normal contact function φLat (α)/φ(α) = 0.85, an angle ϕ = 11◦ , and a ratio cantilever-length to tip-height of L/h = 15 was assumed
70
U. Rabe
the amplitude becomes zero and the phase shifts by −π (Fig. 2.17). This holds also for the slope of the cantilever (not shown here). The solutions for the forced vibration of the complete system according to Fig. 2.8 including lateral forces and tip position can be found in the appendix. A few examples of forced vibration are plotted in Fig. 2.18. The tip position influences the resonant frequencies strongly in all cases, as can be seen in Fig. 2.18a. A shift of the tip from the end position (L 1 /L = 1) to a position only 10% of the length of the beam closer to the fixed end (L 1 /L = 0.9) leads to a dramatic change in the spectrum. The lateral forces influence the spectrum less when the normal contact stiffness divided by the spring constant of the cantilever is lower (k∗ /kC = 100) (b), and they influence the spectrum more when the normal contact stiffness is high (k∗ /kC = 1000) (d). The detector position influences the amplitudes of the measured peaks (c). The first mode, which is not well visible with the beam-deflection sensor at the end of the beam, is much better visible if the detector is located at x = 0.8L. The resonance frequencies do not depend on the detector position, but the frequencies of the anti-resonances depend strongly on the position of the detector on the length axis of the beam. This was also pointed out by Arinero and Lévêque [26].
2.6 Imaging and Contrast Inversion There are different possibilities to evaluate the contact resonances for imaging, as for example amplitude or phase imaging. The cantilever-sample system is excited with a frequency close to a contact resonance [62]. The contact-resonance frequency must be higher than the upper cut-off of the feedback loop. The feedback loop of the AFM works with the quasi static and low frequency components of the cantilever signal and keeps the static deflection of the cantilever at a predefined value while the surface is scanned. Parallel to the topography image the ultrasonic amplitude or phase is measured for example with a lock-in-amplifier and displayed as a color coded image. An example of a topography image and an ultrasonic amplitude image of a piezoelectric ceramic is shown in Fig. 2.19. In the topography image the grains of the polished sample surface can be seen. In the ultrasonic image substructures are visible within the grains which are the ferroelectric domains. The contact stiffness in AFAM and UAFM depends on the orientation of the domains [83, 94]. The contrast of the amplitude images depends strongly on the frequency of operation [95,96] as shown in Fig. 2.20. If the frequency of operation is far from any contact resonance, the contrast vanishes. If the frequency of excitation is lower than the average contact-resonance frequency of the sample, regions with high stiffness will cause lower amplitude of vibration than regions with low stiffness. And if the frequency is higher than the average contact-resonance frequency the contrast inverts. Experimental observation of contrast inversion is an indicator for a contactresonance frequency. It is recommended to operate above the contact-resonance frequency if possible, because the images are more intuitive if surface areas with higher stiffness show higher amplitude of vibration. Imaging of samples with a high variation of Young’s modulus as for example polymer samples with ceramic inclusions will lead to a shift of the contact-resonance
2 Atomic Force Acoustic Microscopy
71
Fig. 2.19. Topography-image (a) and AFAM amplitude-image (b) of a piezoelectric ceramic [82]. The size of the image is 10 × 10 µm2 . The grey scale in the topography image covers 20 nm. The spring constant of the cantilever was 41 N/m. The first two flexural resonant frequencies of the clamped-free beam were 162 kHz and 1004 kHz. The ultrasonic amplitude image was taken above the first contact-resonance frequency at 698 kHz. The white arrows point to a pore in the ceramic surface
Fig. 2.20. Contrast inversion depending on the ultrasonic excitation frequency [95]. A smaller section of the same surface as in Fig. 2.19 was imaged (a) at a frequency below the contactresonance frequency (695 kHz) and (b) above the contact-resonance frequency (699 kHz). The large triangular domain in the middle of the image changes contrast when the frequency of imaging is changed. The principle of contrast inversion is explained in the simulated spectra below. Areas with higher contact stiffness lead to a higher contact-resonance frequency. The dotted lines indicate schematically the frequency of operation below and above the average resonant frequency. The white arrows point to the same pore as seen in Fig. 2.19. The ultrasonic amplitude is always low and contrast inversion is not observed when the tip is on the pore. The topography of the pore leads to a strong variation of contact stiffness and consequently to a contact-resonance frequency much different from the flat areas of the sample
72
U. Rabe
frequency within one image amounting to several multiples of the half-width of the resonant peaks. In this case it is no more possible to find a frequency which is close to the contact-resonance maximum on both phases. Several contrast inversions may happen within one image and the qualitative correspondence between amplitude and stiffness is lost. Strong variations of contact stiffness are also caused by topographical features. One such example can be seen in Fig. 2.20. If the tip is above the small pore in the ceramic which is indicated by white arrows in Fig. 2.19 and Fig. 2.20, the amplitude of vibration is low in both cases of excitation frequency. Probably, the contact-resonance frequency of this area is much different from the contactresonance frequency of the flat surface regions. The contrast in the amplitude images is caused by the shift of the contactresonance frequency with contact stiffness. Furthermore, the amplitude at contact resonance varies with contact stiffness. The theoretical amplitudes at contact resonance of the first three modes are shown in Fig. 2.21. Amplitude or phase imaging is a convenient method to obtain qualitative images of contact-stiffness variation. For quantitative evaluation, however, it is necessary to measure the contact-resonance frequency in every pixel of the image. Kobayashi
Fig. 2.21. Vertical amplitude of the sensor tip dY 0 and lateral amplitude d X0 at the contactresonance frequency of the first three flexural modes as a function of normalized contact stiffness. A detector position at the end of the beam (x = L) was assumed and a low contact damping (γ/(m ∗ ω0 ) = 0.4) was used for the calculation. The curves were obtained by taking the amplitude maxima of simulated contact-resonance curves. All modes have local minima in the lateral amplitude for contact stiffness values at which the slope of the shape function y(x) has local minima at x = L
2 Atomic Force Acoustic Microscopy
73
Fig. 2.22. Topography, height scale 10 nm (a) and contact resonance AFAM-image (b) of nanocrystalline nickel with an average grain size of 167 nm fabricated by pulsed electrodeposition. The sample was polished with diamond paste and alumina solution before imaging [119]. The grey scale of the contact-resonance image ranges from 730 kHz to 750 kHz. The size of the images is 1.5 × 1.5 µm2
et al. developed a phased-locked-loop for the UAFM in order to follow the contactresonance frequency during imaging [97]. The technique was enhanced by amplitude detection by Yamanaka et al. [98]. Fukuda et al. showed that the Q-control technique [99] which was originally developed for tapping mode AFM can also be applied in UAFM [100]. Fast computers and high storage capacities make it possible to sweep spectra in every image point to track the contact-resonance frequency [101, 102] or to save full vibration spectra in every image point (Solver and Ntegra, NT-MDT, Moscow, Russia). The velocity of imaging is only limited by the frequency of vibration and by the contact damping. If contact resonances between 100 kHz and 1 MHz are measured, an image of 128 × 128 pixels takes about half an hour. Topography and contact-resonance frequency images of a nanocrystalline nickel sample are shown in Fig. 2.22. The sample was polished before imaging. The average grain size of the material was 167 nm.
2.7 Sensitivity of the Flexural Modes The influence of the forces which act upon the sensor tip is different for different modes because the mode shape and the wavelength depend on the mode number. In case of quantitative evaluation, the frequency shift of the contact resonances is relevant. The derivative ∂ f/∂k∗ was calculated analytically by Turner and Wiehn [65]. Normalized quantities marked with the symbol “∧” are used here to shorten the calculations: kˆ =
k∗ , kc
kˆ Lat =
∗ kLat , kc
fˆ =
f f 1,free
,
(2.58)
and abbreviations for combinations of the trigonometric and hyperbolic functions which appear frequently are introduced:
74
U. Rabe
ssh(x) = sin(x) sinh(x) cch(x) = cos(x) cosh(x) cch ± (x) = 1 ± cos(x) cosh(x) mix ± (x) = sin(x) cosh(x) ± cos(x) sinh(x)
(2.59)
The dimensionless wave number ψ is defined as ψ = αL. The characteristic equation is a function of the wave number, the contact stiffness and the contact damping. The characteristic equation (2.39) is rewritten in normalized quantities, and only the dependency on the normalized contact stiffness kˆ ∗ is considered: & ' Ω ψ(kˆ ∗ ), kˆ ∗ = 0 (2.60) The derivative of this equation with respect to kˆ ∗ yields [65]: dψ ∂Ω =− ∗ ˆ dk ∂ kˆ ∗
∂Ω ∂ψ
−1 (2.61)
If this formula is applied for example to the characteristic equation of the springcoupled cantilever (2.42) one obtains: −3mix − (ψ) dψ = dkˆ ∗ 3ψ 2 cch + (ψ) − ψ 3 mix − (ψ) + 6kˆ ∗ ssh(ψ)
(2.62)
As the sensitivity is given by the shift of the resonant frequency and not by the shift of the dimensionless wave number, the chain rule and the dispersion relation (2.10) are used: ∂ fˆ ∂ fˆ ∂ψ = ∂ψ ∂ kˆ ∗ ∂ kˆ ∗
∂ fˆ ψ =2 ∂ψ (1.8751)2
(2.63)
Now, the sensitivity σ can be calculated: σ=
−6ψmix − (ψ) d fˆ = dkˆ ∗ (1.8751)2 [3ψ 2 cch + (ψ) − ψ 3 mix − (ψ) + 6kˆ ∗ ssh(ψ)]
(2.64)
To evaluate the sensitivity, the normalized wave number or the contact-resonance frequency is first determined using the characteristic equation (2.42). Afterwards, (2.64) is applied. The sensitivity of the first four flexural modes of the spring-coupled cantilever is shown in Fig. 2.23. In the limit of vanishing contact stiffness (kˆ ∗ = 0) the normalized wave number is ψ = 1.8751 and cch + (1.8751) = 0. Therefore the sensitivity of the first flexural mode is in the limit kˆ ∗ = 0: d fˆ 6 ∗ n = 1 : σ(kˆ = 0) = = ≈ 0.5 (2.65) 4 ∗ ˆ (1.8761) dk ∗ k =0
2 Atomic Force Acoustic Microscopy
75
In general one obtains for the n’th mode in the limit kˆ ∗ = 0: 6 d fˆ = 2 ∗ ˆ (1.8761) (ψn,free )2 dk ∗
(2.66)
k =0
For each value of the contact stiffness one can determine a flexural mode with highest sensitivity. The approximate crossing points of the sensitivity curves in Fig. 2.23 are listed in Table 2.4. The higher the contact stiffness, the higher is the most sensitive mode. The acoustic impedance at the sensor-tip position increases with the mode number [70]. One can also say that the dynamic load which is imposed by the cantilever onto the sample increases with increasing frequency proportional m ∗ ω2 y(L) [27, 29]. However, the maximal value of the sensitivity σ ≈ 0.5 is only reached by the first mode for small contact stiffness (k∗ → 0). This means that the sensitivity can be improved by using higher modes, but the sensitivity of the higher modes of a soft beam will be smaller than the sensitivity of the first mode
Fig. 2.23. Sensitivity σ of the first four flexural modes as a function of normalized contact stiffness [65]. The dashed line shows the sensitivity according to the equivalent point-mass model Table 2.4. Linear model of the cantilever when the sensor tip is in contact with a sample surface. The tip–sample interaction forces are represented by springs and dashpots. The cantilever is tilted by an angle ϕ with respect to the surface. The sensor tip of height h is located at a position L 1 on the length axis of the cantilever. The distance of the tip to the free end of the cantilever is L 2 Mode number n Slope at x = L becomes zero Mode (n + 1) becomes more sensitive than mode n Sensitivity of n’th flexural mode for k∗ → 0
1 k∗ /kC = 9.5 k∗ /kC ≈ 9.9 σ ≈ 0.09 σ = 0.485
2 k∗ /kC = 83 k∗ /kC ≈ 69 σ ≈ 0.04 σ = 0.077
3 k∗ /kC = 279 k∗ /kC ≈ 216 σ ≈ 0.02 σ = 0.028
76
U. Rabe
of a stiffer beam. Unfortunately, a stiffer beam makes the control of the static force more difficult. As the static force is also an important parameter, the choice of the optimal cantilever is always a compromise. Using the Rayleigh–Ritz method, Turner and Wiehn calculated an approximate formula for the sensitivity of the first five flexural and torsional modes [65]. This solution can also be applied to cantilevers with variable cross-section as for example V-shaped beams. The analytical formula of Turner and Wiehn was extended to contact damping by Chang et al. [103]. They found that the contact damping reduces the sensitivity of the modes for small values of contact stiffness k∗ . Furthermore the influence of lateral forces and tilt [104] and the length of the sensor tip [91] were examined. As the contact stiffness depends on the radius of the sensor tip and the Young’s moduli of tip and surface, it is not possible to calculate general formulas for the sensitivity as a function of Young’s modulus of the sample. For such a calculation one must assume a certain tip radius, elastic modulus and static force [96].
2.8 Quantitative Evaluation The characteristic equation derived in Chap. 4 can be solved for an analytical expression which describes the normalized contact stiffness k∗ /kC as a function of contact resonance. The ratio cP between lateral and normal contact function is defined as: cP =
φLat (α) φ(α)
(2.67)
Substituting the auxiliary functions X, T , U (2.38) in the characteristic equation (2.39, 2.40), one obtains a quadratic equation in the contact function φ(α): h2 h φ(α) sin2 ϕ + cP cos2 ϕ + L 21 S2 φ(α) sin ϕ cos ϕ [cP − 1] 2 L1 L1 2 2 h (2.68) + L 1 S1 φ(α) cos ϕ + cP sin2 ϕ + S0 2 φ2 (α)cP = 0 L1
L 41 S4 + L 31 S3
The quadratic term in φ(α) vanishes if there are no lateral forces (cP = 0). If the cantilever is parallel to the sample surface (ϕ = 0), one obtains the following solution for the contact function φ(α): φ(α) = −
L 41 S4 2(αL 1 )3 cch + (αL) = L 1 S1 cch − (αL 1 )mix − (αL 2 ) − cch + (αL 2 )mix − (αL 1 )
(2.69)
In the experiment a contact-resonance frequency f Cont is measured. If the resonant frequencies of the free cantilever are known, the dispersion relation (2.10) containing the measurable quantities can be used to calculate the wave numbers from the measured contact-resonance frequencies: αn,free L f Cont = cn f Cont αL = f n,free
αn,free L with cn := f n,free
(2.70)
2 Atomic Force Acoustic Microscopy
77
In case of small contact damping, its influence on the contact-resonance frequency can be neglected, and the contact function reduces to φ(α) ≈ 3k∗ /kC . One obtains an analytical formula to calculate the normalized contact stiffness k∗ /kC directly from the contact-resonance frequencies [105]. √ √ k∗ (cn f n )3 cch + (cn f n ) (2.71) =3 √ √ kC cch − (cn √f n L 1 /L)mix − (cn √f n L 2 /L) −cch + (cn f n L 2 /L)mix − (cn f n L 1 /L) However, the position of the sensor-tip is usually not known. If one measures the contact-resonance frequencies of two flexural modes and assumes that the contact stiffness is the same for both modes, one can calculate the sensor-tip position numerically [105]. If lateral forces are considered, the quadratic equation must be solved: " L 2 L 4 S4 φ(α) = g ± g2 − 21 1 h S0 cP L 1 S1 (cos2 ϕ + cP sin2 ϕ) + L 21 S2 Lh1 (cP − 1) sin ϕ cos ϕ 2
g=−
+L 31 S3 Lh 2 (sin2 ϕ + cP cos2 ϕ) 1
2
2S0 Lh 2 cP
(2.72)
1
Here g is only an auxiliary quantity. In principle the normalized contact stiffness k∗ /kC can again be calculated if the contact damping is low. However, the tilt angle ϕ of the cantilever, the height h of the sensor tip with relation to the ∗ /k∗ of lateral to normal cantilever length L, and the ratio cP = φLat /φ ≈ kLat contact constants must be known. The tilt angle ϕ is technically defined by the cantilever holder in the AFM. The height of the sensor tip is usually specified by the manufacturer of the commercial probes. The length of the cantilever beam can be measured with an optical microscope. A more precise measurement of the tip height is only possible with a scanning electron microscope. Instead of calculating the contact stiffness from the contact-resonance frequencies, one can also use the formulas for the forced vibration and fit the experimental resonances to the theoretical curves by parameter variation [60, 90]. Because of the various unknown parameters, however, the error in the obtained contact stiffness values can be high. In contrast to the other parameters, the ratio between the lateral and the normal stiffness cP is not a parameter of the instrument, but depends on the elastic constants of the sensor tip, on the local elastic constants of the sample, and the other tip–sample interaction forces. If cP is unknown, care should be taken to work in the range of the dispersion curves where the influence of the lateral forces is low (see Chap. 4.1). The lateral forces shift the resonant frequencies of the modes in a different way than the normal forces. Therefore it should be possible to determine normal and lateral contact stiffness by fitting the measured spectra to the simulated spectra. However, up to now, as discussed in Chap. 2.3, real cantilever beams do not agree perfectly with the analytical model. On the other hand, the lateral contact stiffness can in
78
U. Rabe
principle be measured if torsional or lateral contact-resonance experiments are made at the same location of the sample. 2.8.1 Experiments for Quantitative Evaluation For quantitative evaluation the resonant frequencies of the clamped-free beam are needed. As far as the bandwidth is sufficient the free resonant frequencies can be measured with the internal sweep programs of the commercial instruments. Alternatively an optical interferometer as described in Chap. 2.3 can be used. Two flexural modes are necessary at minimum. However, it is better to determine the resonant frequencies of more flexural modes in order to test how much the cantilever deviates from the model of the clamped-free beam. Then the sensor tip is brought into contact with a sample and a predefined static deflection is set by the operator. The contact-resonance frequencies of at least two modes are measured by sweeping the frequency with the help of the AFAM or UAFM set-up described in Chap. 2. The amplitude of excitation should be kept as small as possible in order to avoid nonlinearities in the spectrum. As contact-resonance frequencies use to shift as a function of applied load, variation of the applied static load helps to distinguish contact resonances from other signals. An example of contact-resonance spectra of three flexural modes and with three different static deflections of the cantilever is shown in Fig. 2.24.
Fig. 2.24. Contact-resonance spectra measured with a silicon cantilever of 41 N/m spring constant on a silicon single crystal [103]. The resonances of the clamped-free beam and contact resonances of the first three flexural modes are shown. The static load for the contact resonances was 410 nN, 820 nN, and 1230 nN. It can be seen that all contact-resonance frequencies are higher than the corresponding free resonance and that the contact-resonance frequencies increase with increasing static load
2 Atomic Force Acoustic Microscopy
79
The sensor-tip position L 1 on the length axis of the cantilever is then calculated numerically. It is assumed that the normalized contact stiffness which is calculated using (2.71) or (2.72) from the measured contact-resonance frequencies must be the same for all contact modes if the static load is identical. If more than two modes are measured, the obtained tip position will in most cases be different for each pair of modes. These differences yield the systematic error in the normalized contact stiffness k∗ /kC which typically amounts to 20% up to 40% at present. The systematic error is caused by the deviation of the real cantilever from the analytical model. After having determined the normalized contact stiffness one has to apply a model for the tip–sample force interaction to obtain an elastic constant of the surface. An elastic constant of the sample surface can be calculated from k∗ /kC using the contact mechanical formulas (2.19) and (2.20) or (2.23), if the spring constant of the cantilever, the normal load, and the elastic constants of the sensor tip and its radius are known. Usually these constants are not known precisely enough, and reference measurements on samples with known elastic constants are necessary. Figure 2.25 shows a sequence of measurements on two silicon single crystal surfaces with different orientation [82]. A reproducible difference between the contact-resonance frequencies of the two surfaces is visible, but also an average increase in the contactresonance frequencies and in the contact stiffness. The increase in contact stiffness is caused by tip wear [62, 79, 106]. Often the contact-resonance frequency increases strongly during the first measurements. A more stable situation is reached after the tip has been rounded so much that the pressure in the contact area is reduced sufficiently to stop further tip damage. The different symbols in Fig. 2.25 belong to different static cantilever loads. As can be seen, the static force has a strong influence
Fig. 2.25. Sequence of contact-resonance measurements on two different silicon single crystal surfaces of different orientation [82]. The contact-resonance frequencies of the first two flexural modes are shown (a) and (b). Four different static loads of the cantilever, 420 nN, 840 nN, 1260 nN, and 1680 nN were chosen. The contact stiffness k∗ calculated from (a) and (b) is shown (c). The cantilever made of silicon single crystal with the dimensions 120 × 30 × 2.8 µm3 (length × width × thickness) had a spring constant of 42 N/m. The first two clamped-free resonant frequencies of the sensor were 287.96 kHz and 1596.37 kHz
80
U. Rabe
on the contact-resonance frequency. The shift of the contact stiffness as a function of applied load can be used to estimate the shape of the sensor tip [56]. If the sensor tip is broken, so that the end of the tip is flat, the contact-resonance frequencies do not shift any more as a function of applied load. A flat tip could be an advantage, because in this case the contact area would be constant and known. On the other hand it is difficult to align a flat tip parallel to the sample surface. By comparison of the normalized contact stiffness on the two samples, the difference of the elastic constants can be calculated. When the normal load Fn and the tip radius R are identical for a measurement on a sample of interest and on a reference sample, one can conclude from the Hertzian model, (2.19): " k∗3 ∗ ∗ E = E Ref · (2.73) ∗ 3 kRef ∗ ∗ and kRef are the reduced Young’s modulus and the contact stiffness of the Here E Ref ∗ ∗ · k∗ /kRef , holds in reference sample, respectively. A simpler expression, E ∗ = E Ref the case of a flat tip. The indentation modulus of the sample MS can be calculated by solving (2.23): MS−1 = E ∗−1 − MT−1 . In case of an isotropic sample with known Poisson’s ratio the Young’s modulus follows directly from MS using (2.20). The indentation modulus of the tip can be calculated from the elastic single crystal constants of the tip material if they are known, or it can be measured using two reference samples: ( M1 M2 1 − k1∗3 /k2∗3 ( (2.74) MT = M2 k1∗3 k2∗3 − M1
Here M1 , M2 , k1∗ , and k2∗ are the indentation modulus and the contact stiffness of reference samples 1 and 2, respectively. The steps for quantitative measurements are summarized schematically in Fig. 2.26. By comparison of the contact stiffness on two samples the difference in the elastic constants can be determined. The elastic contact generates shear stresses and compressional stresses in the tip and the sample. The anisotropy in the indentation
Fig. 2.26. Schematic list showing the measurements and steps of evaluation which are necessary to obtain quantitative elastic constants of a sample surface
2 Atomic Force Acoustic Microscopy
81
modulus is therefore lower than the anisotropy in the Young’s modulus. It was shown for silicon single crystal surfaces with two different orientations that the measured difference in contact stiffness k∗ agreed with the difference in k∗ predicted by the indentation modulus calculated from the elastic single crystal constants of silicon [82]. Nanocrystalline ferrites [105], diamond like carbon thin films [79], and clay minerals [107] were examined by contact-resonance spectroscopy. Figure 2.27 shows contact-resonance spectra on polystyrene, clay, mica and fused silica [107]. Polystyrene and fused silica were chosen as reference materials. Clay minerals fill the pores between fused silica grains in sandstone. They influence the average elastic constants of sand stone strongly, but measurement of their elastic constants is not easy. With the AFAM-measurements it was possible to estimate the Young’s modulus of the clay minerals. Dupas et al. imaged WC and Co-Phases in WC-Co Cermets and examined NiTi-epoxy composites by contact-resonance spectroscopy. They obtained quantitative results by fitting the measured spectra to simulations [60]. Hurley et al. examined the elastic constant of a niobium film quantitatively by AFAM [64], and Hurley and Turner investigated the influence of ambient humidity on quantitative AFAM results [108]. Piezoelectric ceramics like BaTiO3 and PZT were investigated by AFAM and the domain contrast was examined [83]. The indentation modulus of BaTiO3 ceramics and PZT ceramics was calculated and compared to experiments [83]. Tsuji et al. evaluated the stiffness of domain boundaries in piezoelectric material by UAFM [109]. Up to the present, commercially available cantilevers have large tolerances in their dimensions and they do not behave perfectly like a clamped beam. Therefore reliable quantitative measurements are only possible if one chooses reference samples with elastic constants close to the constants of the sample of interest. In addition, the error in the obtained values for the elastic constants depends on the control of the static load. It is essential for the calibration by reference sample to compare measurements that are made with the same normal load. In most commercial instruments, however, there is no possibility to apply a calibrated force to the cantilever.
Fig. 2.27. Contact-resonance spectra on polystyrene, clay, mica and fused silica [104]. The spectra of the first and the second contact-resonance frequency of a cantilever with a spring constant of 1.5 N/m are shown
82
U. Rabe
Fig. 2.28. Contact stiffness image of a nanocrystalline nickel sample. The contact stiffness values were calculated from contact-resonance frequencies. The size of the image is 1.5 × 1.4 µm2 . The spring constant of the employed cantilever was 48 N/m and its free resonant frequencies were 166 kHz and 1031 kHz for the first and the second flexural mode, repectively
The force is applied indirectly by approaching the sample and the fixed end of the cantilever. Due to the tilt of the cantilever with respect to the surface, the cantilever buckles and the static bending depends on the normalized contact stiffness k∗ /kC . Because of the different amount of buckling identical static beam-deflection signals do not correspond to identical normal loads Fn if the elastic constants of the samples differ strongly. With the new imaging techniques discussed in Chap. 6 it is possible to obtain contact-resonance images instead of only amplitude images. From two resonant frequency images of two different modes one can calculate a contact stiffness image as shown in Fig. 2.28 and an indentation modulus image if reference measurements are available [101, 102].
2.9 Nonlinear Forces A simple force curve contains an attractive adhesive part and a repulsive elastic part [110,111]. In AFM in air, adhesion forces caused by a water meniscus dominate and drop almost to zero when the water meniscus breaks. When the amplitude of vibration is slowly increased, the nonlinearity of the force is more and more sensed by the AFM. The resonance curves develop a steep edge at the left side of the spectrum, the maximum shifts to lower frequencies and an amplitude jump is noticed with hysteresis when the direction of the frequency scan is inverted [62]. An example of contact-resonance spectra measured with different amplitudes of excitation is shown in Fig. 2.29. It has been shown that the contribution of the local elasticity and the adhesion to the contact forces can be separated by exploiting the amplitude dependence of the resonant frequency, the so-called backbone curve [112]. In the regime of small nonlinearity, when the tip remains in contact with the sample surface during its vibration cycle, the cantilever vibration behavior resembles that of a macroscopic Hertzian contact oscillator [113]. The harmonic balance method [112] or the multiple scales technique [74] can be applied to solve the equation of motion approximately. Amplitude jumps caused by bistability are typical for a nonlinear system with softening behavior [114]. If the amplitude of surface vibration is increased, one can observe that the high frequency amplitude of the cantilever first increases linearly. After a certain thresh-
2 Atomic Force Acoustic Microscopy
83
Fig. 2.29. Contact-resonance spectra showing the influence of the nonlinear forces [62]. (a) When the excitation amplitude of the transducer is increased, the spectra become asymmetric and develop a steep edge. (b) Hysteresis depending on the direction of the frequency scan
old, however, the minimum of the force curve is passed through during a vibration cycle and the amplitude of vibration of the cantilever remains constant or even decreases [115]. At the same time a DC offset of the cantilever develops, i.e. the sensor tip lifts off the sample surface. In this amplitude region UFM and SAFM are operating. At very high amplitudes the tip jumps so far away from the sample surface that the water meniscus breaks and the interaction forces drop almost to zero during a vibration cycle. The contact with the sample can now be considered as an impact where the impact time is short compared to the period of oscillation. In this regime subharmonics have been observed [116] and the ultrasonic mode resembles the intermittent contact or tapping mode where the vibration is excited by the transducer in the cantilever holder. Different authors have examined the influence of the nonlinear forces on the spectrum of the first flexural resonance in the tapping mode and in the non-contact mode [117–119]. Recently Stark et al. applied a state-space model to examine flexural vibration spectra in the tapping mode including the higher modes [120].
2.10 Conclusions Analytical models to describe flexural cantilever vibration for quantitative measurement of elastic constants have been summarized in this article. Examples of application by different research groups have been given. The challenge in quantitative AFAM will be to manufacture and model sensors in such a way that a characterization of every individual sensor by electron microscopy is not necessary. Furthermore, sensor tips with a well defined radius, a high stiffness and a high resistance to breaking and wear must be developed. Imaging techniques which acquire the contact-resonance frequency or full spectra in every point of the surface are more favorable than mere amplitude or phase imaging. Such techniques will make it possible to map local surface stiffness and contact damping quantitatively. In cases where high local resolution is not required, the precision of nanoindentation with regard to quantitative Young’s modulus will probably be higher, because nanoindentation provides calibrated force measurements and forces
84
U. Rabe
normal to the surface. On the other hand, the development of contact mechanics models for dynamic indentation is an active area of research, where nanoindentation and the AFM-techniques can stimulate each other. The potential of the high frequency AFM techniques like AFAM and UAFM is local resolution in the nm-range which can in principle be achieved, the possibility of fast image acquisition and the possibility to examine frequency-dependent phenomena. Furthermore, the measurement of frequencies is an advantage, as it avoids difficult calibration of amplitude. By combination of the results from different bending, lateral bending and torsional modes, elastic constants in three directions relative to the sample surface can be measured by AFM. Nonlinear tip–sample forces such as friction and adhesion change the shape of the resonance curves in a characteristic way. Quantitative evaluation of nonlinear resonance curves is a still larger challenge than elasticity measurement. Numerical modeling and absolute measurement of the vibration amplitudes of tip and sample will be required in this case. Acknowledgements. The author would like to thank W. Arnold, all colleagues, coworkers, and students for support and collaboration. Critical proofreading of this manuscript by S. Hirsekorn is gratefully acknowledged. Part of this work was supported by the German ministry of education and research (BMBF) in the frame of the research program “Nanoanalytik” under the contract No. FKZ13N8326.
A Appendix A.1 Definitions In order to calculate the forced vibration for the model shown in Fig. 2.8, including the angle ϕ of the cantilever, lateral forces, and tip position, abbreviations are defined for combinations of the trigonometric and hyperbolic functions which are needed frequently: s1± = sin αL 1 ± sinh αL 1
s2± = sin αL 2 ± sinh αL 2
± c± 1 = cos αL 1 ± cosh αL 1 c2 = cos αL 2 ± cosh αL 2 ssh 1 = sin αL 1 sinh αL 1 ssh 2 = sin αL 2 sinh αL 2 cch 1 = cos αL 1 cosh αL 1 cch 2 = cos αL 2 cosh αL 2
cch ± 1 = 1 ± cos αL 1 cosh αL 1
cch ± 2 = 1 ± cos αL cosh αL
cch + 1+2 = 1 + cos α(L 1 + L 2 ) cosh α(L 1 + L 2 ) mix1± = sin αL 1 cosh αL 1 ± cos αL 1 sinh hαL 1 mix2± = sin αL 2 cosh αL 2 ± cos αL 2 sinh hαL 2
(A.1)
As can be seen in Table 2.3, the formulas for the forced vibration excited by a concentrated force acting at the free end of the beam are very similar to the solutions in
2 Atomic Force Acoustic Microscopy
85
Table 2.3 case (b), excitation by surface vibration. Therefore only the UAFM-mode and AFAM-mode are calculated here. In both cases, the calculation is based on the equation of motion (2.1), the dispersion relation (2.5) and the solution (2.3). The definitions of the contact functions φ(α) and φLat (α), the dimensionless contact damping p and the auxiliary functions X, T , and U in (2.33)–(2.38) are not repeated here. They can be taken from the main body of the text. As discussed in Chap. 4, two functions y(x) and y2 (x2 ) are defined for the two sections of the beam from the clamped end to the tip position and from the free end to the tip position, respectively. A.2 UAFM-mode In case of a vertical vibration of the clamped end of the beam the boundary conditions are: ⎧ 2 ∂ y2 (x2 ) ⎪ ⎪ =0 ⎨ (x) = u 0 ∂x22 x = 0 : ∂y(x) x2 = 0 : 3 ∂ y2 (x2 ) ⎪ =0 ⎪ ⎩ =0 ∂x ∂x23 ⎧ ⎨ y(x) = y2 (x2 ) ∂y2 (x2 ) x = L 1 or x2 = L 2 : ∂y(x) =− ⎩ ∂x ∂x2 ⎧ 2 2 ∂y(x) ∂ y(x) ∂ y2 (x2 ) ⎪ ⎪ − = −T(α) − X(α)y(x) ⎨ ∂x 2 ∂x ∂x22 x = L 1 or x2 = L 2 : ∂y(x) ∂ 3 y(x) ∂ 3 y2 (x2 ) ⎪ ⎪ ⎩ + = U(α) · y(x) + X(α) 3 3 ∂x ∂x ∂x2 (A.2) By combining the functions y(x) andy2 (x2 ) and the first four boundary conditions one obtains: u0 y(x) = (cos αx + cosh αx) + A2 (cos αx − cosh αx) + A4 (sin αx − sinh αx) 2 (A.3) y2 (x2 ) = A1 (cos αx2 + cosh αx2 ) + A3 (sin αx2 + sinh αx2 ) The remaining four boundary conditions together with these solutions lead to a linear system of equations with four unknown constants A1 , A2 , A3 and A4 . Solving the linear system for the constants leads to: *
+ + u0 ) + − + − 4 + + 3 2 −2α5 c− 1+2 − α Tc2 s1 + α X s2 s1 + c2 c1 − α Us2 c1 N(α)
u0 ) 5 2α ssh 1+2 + α4 T ssh 1 mix2+ + mix1− cch + A2 = 2 N(α)
− + + 2 −2α3 X ssh 1 ssh 2 + cch 1 cch + 2 + α U ssh 1 mix 2 − mix 1 cch 2 * −α(TU − X 2 )ssh 1 cch + 2 A1 =
86
U. Rabe
*
+ + u0 ) − − + − 4 − + 3 2 −2α5 c− 1+2 − α Ts2 s1 + α X −c2 s1 + s2 c1 + α Uc2 c1 N(α)
u0 ) + + + − α4 T 2ssh 1 cch + A4 = −2α5 mix1+2 2 + mix 1 mix 2 N(α) *
+ (A.4) −2α3 X mix1− cch + 2 − mix 1 ssh 2 A3 =
With the common denominator N(α): + − + + 4 N(α) = 2{−2α5 cch + 1+2 + α T(mix 2 cch 1 − cch 2 mix 1 ) − − − + − 2 − 2α3 X(cch + 2 ssh 1 + ssh 2 cch 1 ) + α U(mix 2 cch 1 − cch 2 mix 1 ) − − α(TU − X 2 )cch + 2 cch 1 }
(A.5)
If the sensor tip is located at the end of the beam (L 2 = 0), the constants and the denominator simplify to: * u0 ) 4 −α ssh − α3 Tmix − + 2α2 Xcch + αUmix + + (TU − X 2 )ssh 2N0 (α) u0 {α4 mix + + 2α3 Tssh + 2α2 Xmix − − 2αUcch A4 = 2N0 (α) − (TU − X 2 )mix + }N0 (α) = α4 cch + + α3 Tmix + + 2α2 Xssh A2 =
+ αUmix − + (TU − X 2 )cch −
(A.6)
The amplitude and the slope at the end of the beam (x = L) are in this case (L 2 = 0): u0 {α4 c+ + α3 Ts+ − α2 Xc− } N0 (α) u0 ∂y (L, α) = α {α4 s− − α2 Xs+ + αUc− } ∂x N0 (α)
y(L, α) =
(A.7)
The forced vibration in the UAFM-mode with lateral forces and tilt of the cantilever, but without variable tip position, was discussed in a publication [121]. Unfortunately, there are several typewriting errors in the formulas in this publication. The correct boundary conditions were published for example in [104]. A.3 AFAM-mode In the case of vibration of the surface in its normal direction, one obtains components of excitation in vertical direction (y-direction) and in lateral direction (x-direction) in the coordinate system of the cantilever. The formulas derived here can also be used for excitation of flexural modes by lateral surface vibration. The components of excitation in the coordinate system of the cantilever need only to be changed in this case. In case of normal surface vibration the boundary conditions are:
2 Atomic Force Acoustic Microscopy
87
⎧ ∂2 y ⎪ ⎪ ⎨ y(x) = 0 =0 2 x = 0 : ∂y(x) y = L : ∂x3 ⎪ =0 ∂ y ⎪ ⎩ ∂x =0 ∂x 3 ⎧ ⎨ y(x) = y2 (x2 ) ∂y2 (x2 ) x = L 1 or x2 = L 2 : ∂y(x) =− ⎩ ∂x ∂x2 ⎧ 2 2 ∂y(x) ∂ y(x) ∂ y2 (x2 ) ⎪ ⎪ − X(α)y(x) − = a0 − T(α) ⎨ ∂x 2 ∂x ∂x22 x = L 1 or x2 = L 2 : ∂ 3 y(x) ∂ 3 y2 (x2 ) ∂y(x) ⎪ ⎪ ⎩ + = −b0 + U(α) · y(x) + X(α) 3 ∂x 3 ∂x ∂x2 (A.8)
With the components of excitation in the coordinate system of the cantilever: a0 = −u 0
h φLat (α) sin ϕ L 31
b0 = u 0
1 φ(α) cos ϕ L 31
(A.9)
Using the first four boundary conditions one obtains the following solutions for the two sections of the cantilever: y(x) = A2 (cos αx − cosh αx) + A4 (sin αx − sinh αx) y2 (x2 ) = A1 (cos αx2 + cosh αx2 ) + A3 (sin αx2 + sinh αx2 )
(A.10)
The constants are again calculated using the four boundary conditions at the tip position and solving the linear system of equations for the constants A1 , A2 , A3 , and A4 : + ) + + − − − + 2 A1 = −α3 a0 c+ 2 ssh 1 + s2 mix 1 + c2 cch 1 − α b0 c2 mix 1 + s2 ssh 1 * + − + − −s2− cch − 1 + α (Xa0 − Tb0 ) c2 cch 1 + (Xb0 − Ua0 ) s2 cch 1 /N(α) ) + + − − − 2 A2 = −α3 a0 mix2+ s1− + ssh 2 c− 1 − cch 2 c1 + α b0 mix 2 c1 + ssh 2 s1 * + + − + − +cch + 2 s1 + α (Xa0 − Tb0 ) cch 2 c1 − (Xb0 − Ua0 ) cch 2 s1 /N(α) + ) + − − − − − 2 A3 = α3 a0 c+ 2 mix 1 − s2 ssh 1 − s2 cch 1 − α b0 −c2 ssh 1 + s2 mix 1 * − − − + − +c− 2 cch 1 + α (Xa0 − Tb0 ) s2 cch 1 − (Xb0 − Ua0 ) c2 cch 1 /N(α) ) + − A4 = α3 a0 −ssh 2 s1+ + mix2+ c− 1 − cch 2 s1 − + + + +α2 b0 −ssh 2 c− 1 + mix 2 s1 − cch 2 c1 * + + − (A.11) +α (Xa0 − Tb0 ) cch + 2 s1 + (Xb0 − Ua0 ) cch 2 c1 /N(α) The denominator N(α) is the same as in the UAFM-mode (A.5). If the position detector is located at the end of the beam (x2 = 0), the solution simplifies to: y2 (0) = 2A1
∂y2 (0) = −2αA3 ∂x2
(A.12)
88
U. Rabe
References 1. Hurley DC, Tewary VK, and Richards AJ (2001) Meas Sci Technol 12:1486 2. Every AG (2002) Meas Sci Technol 13:R21 3. Zieniuk JK and Latuszek A (1989) in: Shimizu H, Chubachi N, Kushibiki J (eds) Acoust Img 17. Plenum Press, New York, p 219 4. Khuri-Yakub BT, Cinbis C, Chou CH, Reinholdtsen PA (1989) in: McAvoy BR (ed) Proc. IEEE Ultrasonics Symp, p 805 5. Kulik A, Attal J, Gremaud G (1993) in: Wei Y and Gu B (eds) Acoustical Imaging 20. Plenum Press, New York, p 241 6. Quate CF, Khuri-Yakub BT, Akamine S, Hadimioglu BB (1994) United States Patent 5,319,977 7. Günther P, Fischer UCh, Dransfeld K (1998) Appl Phys B 48:89 8. Giessibl FJ (1998) Appl Phys Lett 73:3956 9. Binnig G, Quate CF, Gerber Ch (1986) Phys Rev Lett 56:930 10. Kolosov O and Yamanaka K (1993) Jpn J Appl Phys 32:22 11. Chilla E, Hesjedahl T, Fröhlich H-J (1997) Phys Rev B 55:15852 12. Rabe U and Arnold W (1994) Appl Phys Lett 64:1493 13. Yamanaka K and Nakano S (1996) Jpn J Appl Phys 35:3787 14. Rohrbeck W and Chilla E (1992) Phys stat sol (a) 131:69 15. Hesjedahl T and Behme G (2001) Europhys Lett 54:154 16. Yamanaka K, Ogiso H, Kolosov O (1994) Jpn J Appl Phys 33:3197 17. Kolosov OV, Castell MR, Marsh CD, Briggs GAD, Kamins TI, Williams RS (1998) Phys Rev Lett 81:1046 18. Yamanaka K (1996) Thin Solid Films 273:116 19. Inagaki K, Kolosov OV, Briggs GAD, Wright OB (2000) Appl Phys Lett 76:1836 20. Inagaki K, Matsuda O, Wright OB (2002) Appl Phys Lett 80:2386 21. Huey BD (2002) in: Maev RG (ed) Acoust Img 26. Kluver Academic/Plenum Publishers, p 183 22. Dinelli F, Castell MR, Ritchie DA, Mason NJ, Briggs GAD, Kolosov OV (2000) Phil Mag A 80:2299 23. Maivald P, Butt H-J, Gould SAC, Prater CB, Drake B, Gurley JA, Elings VB, Hansma PK (1991) Nanotechnology 2:103 24. Florin E-L, Radmacher M, Fleck B, Gaub HE (1994) Rev Sci Instr 65:639 25. Mazeran P-E and Loubet J-L (1997) Tribol Lett 3:125 26. Arinero R and Lévêque G (2003) Rev Sci Instr 74:104 27. Troyon M, Wang Z, Pastre D, Lei HN, Hazotte A (1997) Nanotechnology 8:163 28. Rosa A, Weilandt E, Hild S, Marti O (1997) Meas Sci Technol 8:1 29. Burnham NA, Kulik AJ, Gremaud G, Gallo PJ, Oulevey F (1996) J Vac Sci Technol B14:794 30. Oulevey F, Gremaud G, Mari D, Kulik AJ, Burnham NA, Benoit W (2000) Scripta mater 42:31 31. Elings VB and Gurley JA (1993) US Patent No. 5,266,801 32. Hirsekorn S, Rabe U, Arnold W (2001) Appl Phys A 72 [Suppl.]:S87 33. Cretin B and Sthal F (1993) Appl Phys Lett 62:829 34. Robert L and Cretin B (1999) Surf Interface Anal 27:568 35. Vairac P and Cretin B (1996) Appl Phys Lett 68:461 36. Cretin B and Vairac P (1997) Appl Phys Lett 71:2082 37. Oliver WC and Pharr GM (1992) J Mater Res 7:1564 38. Lorenz D, Fränzel W, Einax M, Grau P, Berg G (2001) J Mater Res 16:1776 39. Seyed Asif SA, Wahl KJ, Colton RJ, Warren OL (2001) J Appl Phys 90:1192 40. Bushan B and Li X (2003) Int Mater Rev 48:125
2 Atomic Force Acoustic Microscopy
89
41. Butt H-J and Jaschke M (1995) Nanotechnology 6:1 42. Salapaka MV, Bergh HS, Lai J, Majumdar A, McFarland E (1997) J Appl Phys 81:2480 43. Rabe U, Janser K, Arnold W (1996) in: Tortoli P and Masotti L (eds) Acoustical Imaging 22. Plenum Press, New York, p 669 44. Rabe U, Janser K, Arnold W (1996) Rev Sci Instr 67:3281 45. Meyer G and Amer NM (1990) Appl Phys Lett 57:2089 46. Marti O, Colchero J, Mlynek J (1990) Nanotechnology 1:141 47. Kawagishi T, Kato A, Hoshi Y, Kawakatsu H (2002) Ultramicroscopy 91:37 48. Pfeiffer O, Bennewitz R, Baratoff A, Meyer E (2002) Phys Rev B 65:161403 49. Reinstädtler M, Rabe U, Scherer V, Hartmann U, Goldade A, Bushan B, Arnold W (2003) Appl Phys Lett 82:2604 50. Krotil HU, Weilandt E, Stifter Th, Marti O, Hild S (1999) Surf Interface Anal 27:341 51. Caron A, Rabe U, Reinstädtler M, Turner JA, Arnold W (2004) Appl Phys Lett 85:6398 52. Drobeck T, Stark RW, Gräber M, Heckl WM (1999) New J Phys 1:15.1 53. Drobeck T, Stark RW, Heckl W (2001) Phys Rev B 64:045401 54. Yamanaka K and Nakano S (1998) Appl Phys A 66:S313 55. Yamanaka K, Noguchi A, Tsuji T, Koike T, Goto T (1999) Surf Interface Anal 27:600 56. Yamanaka K, Tsuji T, Noguchi A, Koike T, Mihara T (2000) Rev Sci Instr 71:2403 57. Crozier KB, Yaralioglu GG, Degertekin FL, Adams JD, Minne SC, Quate CF (2000) Appl Phys Lett 76:1950 58. Yaralioglu GG, Degertekin FL, Crozier KB, Quate CF (2000) J Appl Phys 87:7491 59. Crozier KB, Yaralioglu GG, Degertekin FL, Adams JD, Minne SC, Quate CF (2000) Proc SPIE 4099:48 60. Dupas E, Gremaud G, Kulik A, Loubet J-L (2001) Rev Sci Instr 72:3891 61. Rabe U and Arnold W (1994) Ann Phys 3:589 62. Rabe U, Kester E, Arnold W (1999) Surf Interface Anal 27:386 63. Stark RW, Drobeck T, Heckl WM (2001) Ultramicroscopy 86:207 64. Hurley DC, Shen K, Jennett NM, Turner JA (2003) J Appl Phys 94:2347 65. Turner JA and Wiehn JS (2001) Nanotechnology 12:322 66. Weaver W, Timoshenko SP, Young DH (1990) Vibration Problems in Engineering. John Wiley, New York 67. Stokey FW (1976) Vibration of Systems Having Distributed Mass and Elasticity. In: Harris CM, Crede CE (eds) Shock and Vibration Handbook, McGraw-Hill, New York, Chapter 7 68. Radmacher M, Tillmann RW, Gaub HE (1993) Biophys J 64:735 69. Burnham NA, Gremaud G, Kulik AJ, Gallo P-J, Oulevey F (1996) J Vac Sci Technol B 14:1308 70. Turner JA, Hirsekorn S, Rabe U, Arnold W (1997) J Appl Phys 82:966 71. Reinstädtler M, Rabe U, Scherer V, Turner JA, Arnold W (2003) Surf Sci 532-535:1152 72. Hoummady M, Farnault E, Yahiro T, Kawakatsu H (1997) J Vac Sci Technol B 15:1539 73. Monchalin J-P (1986) IEEE Transactions UFFC-33:485 74. Turner JA and Hurley DC (2003) Instrumentation, Mesure, Métrologie 3:117 75. Reinstädtler M (2004) Elastische und tribologische Oberflächencharakterisierung auf der Nanoskala mittels Torsions- und Lateralmoden von Sensorbalken der Rasterkraftmikroskopie. PhD Thesis, Naturwissenschaftlich-Technische Fakultät III der Universität des Saarlandes, unpublished 76. Pietrement O and Troyon M (2000) J Colloid and Interface Science 226:166 77. Schwarz UD (2003) J Colloid and Interface Science 261:99 78. Johnson KL (1985) Contact mechanics. Cambridge University Press, Cambridge 79. Amelio S, Goldade AV, Rabe U, Scherer V, Bushan B, Arnold W (2001) Thin solid films 392:75 80. Pharr GM, Oliver WC, Brotzen F (1992) J Mat Res 7:613
90
U. Rabe
81. Vlassak JJ and Nix WD (1993) Phil Mag A67:1045 82. Rabe U, Amelio S, Kopycinska M, Hirsekorn S, Kempf M, Göken M, Arnold W (2002) Surf Interface Anal 33:65 83. Rabe U, Kopycinska M, Hirsekorn S, Muñoz Saldaña J, Schneider GA, Arnold W (2002) J Phys D: Appl Phys 35:2621 84. Sarioglu AF, Atalar A, Degertekin FL (2004) Appl Phys Lett 84:5368 85. Tsuji T and Yamanaka K (2001) Nanotechnology 12:301 86. Tsuji T, Irihama H, Yamanaka K (2002) JSME Int J A 45:561 87. Tsuji T, Irihama H, Yamanaka K (2002) Jpn J Appl Phys 41:832 88. Yamanaka K, Tsuji T, Irihama H, Mihara T (2003) Proc SPIE 5045:104 89. Wright OB and Nishiguchi N (1997) Appl Phys Lett 71:626 90. Dupas E (2000) Cartographie et spectroscopie des propriétés méchaniques à l’échelle du nanomètre par spectrométrie acoustique locale à fréquence variable: Thèse no 2278, EPFL Lausanne, unpublished 91. Wu T-S, Chang W-J, Hsu J-Ch (2004) Microelectronic Engineering 71:15 92. Muraoka M (2002) JSME Int J A 45:567 93. Muraoka M (2005) Nanotechnology 16:542 94. Karapetian E, Kachanov M, Kalinin SV (2005) Phil Mag 85:1017 95. Rabe U, Amelio S, Hirsekorn S, Arnold W (2000) in: Halliwell M and Wells NT (eds) Acoust Img 25. Kluwer Academic/Plenum, New York, p 253 96. Rabe U, Amelio S, Kester E, Scherer V, Hirsekorn S, Arnold W (2000) Ultrasonics 38:430 97. Kobayashi K, Yamada H, Matsushige K (2002) Surf Interface Anal 33:89 98. Yamanaka K, Maruyama Y, Tsuji T, Nakamoto K (2001) Appl Phys Lett 78:1939 99. Anczykowski B, Cleveland JP, Krüger D, Elings V, Fuchs H (1998) Appl Phys A 66:S885 100. Fukuda K, Irihama H, Tsuji T, Nakamoto K, Yamanaka K (2003) Surf Sci 532-535:1145 101. Hurley DC, Kos AB, Rice P (2005) Mater Res Soc Proc 838E:08.2.1 102. Hurley DC, Kopycinska-Müller M, Kos AB, Geiss RH (2005) Adv Eng Mat 7:713 103. Chang W-J, Fang T-H, Chou H-M (2003) Phys Lett A 312:158 104. Chang W-J (2002) Nanotechnology 13:510 105. Kester E, Rabe U, Presmanes L, Tailhades Ph, Arnold W (2000) J Phys Chem Solids 61:1275 106. Kopycinska-Müller M, Geiss RH, Rice P, Hurley DC (2005) Mater Res Soc Proc 838E:010.16.1 107. Prasad M, Kopycinska M, Rabe U, Arnold W (2002) Geophys Research Lett 29:13-1 108. Hurley DC and Turner J (2004) J Appl Phys 95:2403 109. Tsuji T, Ogiso H, Akedo J, Saito S, Fukuda K, Yamanaka K (2004) Jpn J Appl Phys 43:2907 110. Hirsekorn S, Rabe U, Arnold W (1996) Europhysics News 27:93 111. Hirsekorn S, Rabe U, Arnold W (1997) Nanotechnology 8:57 112. Muraoka M and Arnold W (2001) JSME Int J A 44:396 113. Turner JA (2004) J Sound and Vibration 275:177 114. Nayfeh AN and Mook DT (1979) Nonlinear Oscillations. Wiley, New York 115. Hirsekorn S, Rabe U, Arnold W (1997) Nanotechnology 8:57 116. Burnham NA, Kulik AJ, Gremaud G (1995) Phys Rev Lett 74:5092 117. Wang L (1998) Appl Phys Lett 73:3781 118. Sasaki N and Tsukuda M (1999) Appl Surf Sci 140:339 119. Lee SI, Howell SW, Raman A, Reifenberger R (2002) Phys Rev B 66:115409 120. Stark RW, Schitter G, Stark M, Guckenberger R, Stemmer A (2004) Phys Rev B 69:085412 121. Rabe U, Turner J, Arnold W (1998) Appl Phys A 66:S277 122. Kopycinska-Müller, M (2005) PhD-Thesis, Naturwissenschaftlich-Technische Fakultät III der Universität des Saarlandes, unpublished
3 Scanning Ion Conductance Microscopy Tilman E. Schäffer · Boris Anczykowski · Harald Fuchs
3.1 Introduction The era of scanning probe microscopy was launched in 1981 with the construction of the first scanning tunneling microscope (STM) by Binnig, Rohrer and coworkers [1]. This microscope is based on the measurement of tiny tunneling currents between a sharp metal probe and a flat metal sample. For the first time, individual atoms could be laterally resolved on conducting surfaces. But more than that, the STM has triggered the development of a large family of new microscopes, the so-called scanning probe microscopes (SPM), that are all based on a small, locally confined probe which is sensitive to various kinds of physical quantities. In 1984, Pohl et al. invented the near-field scanning probe microscope (NSOM) that enables optical imaging of surfaces with sub-wavelength resolution [2]. In 1986, in the same year when they received the Nobel Price for their development of the STM, Binnig et al. invented the atomic force microscope (AFM) [3]. This microscope is based on the measurement of minute forces. One of its main applications is the creation of highresolution topographic images of surfaces, where it has the advantage over STM of not requiring conducting probes and samples. The additional benefit of the AFM that it can image in different environmental conditions including aqueous buffer solution makes it well suited for biological applications [4]. Several related scanning probe microscopes have been developed so far, including the magnetic force microscope (MFM) [5, 6], the electric force microscope [7] and the scanning electrochemical microscope (SECM) [8]. In this chapter, we focus on the scanning ion conductance microscope (SICM), which was invented by Hansma et al. in 1989 [9, 10]. The SICM records the ionic current through a small aperture as this aperture is scanned over the surface of a sample immersed in an electrolyte solution. The aperture is usually formed by a nanopipette. Two electrodes are placed in the electrolyte: one inside the pipette (pipette electrode), and one outside the pipette in the bath over or under the sample (bath electrode). By applying a voltage between both electrodes and recording the ion current through the pipette, locally resolved images of the ion current over the sample surface can be generated. Despite the many possible applications of such a microscope, the SICM is one of the least developed scanning probe microscopy technique so far. Only few setups are described in literature [9–17]. Most researchers have used drawn-out glass capillaries as pipettes similar to those used in intracellular recording and patch clamp experiments [18,19], but some also used microfabricated probes [20]. Typical opening diameters of the tips of the
92
T.E. Schäffer · B. Anczykowski · H. Fuchs
glass nanopipettes are 30–100 nm, and lateral scan resolutions in the same range are obtained. There is a strong dependence of the measured current on the tipsample distance (“current squeezing effect”). The tip-sample distance can therefore be kept constant during scanning by using the current as an input to a feedback loop, thereby generating images of sample topography. This particularly works for non-porous samples where the bath electrode is positioned on the same side of the sample as the pipette. Pipette and sample do not come into mechanical contact with each other, and soft and delicate samples such as living cells can be imaged in this “non-contact” configuration [14]. To improve the imaging capabilities of the SICM, several methods have been devised that are mostly based on the principle of an ac measurement. By modulating either the pipette current or the tip-sample distance and by using lock-in amplifiers, these methods exhibit several advantages over the regular dc method [16, 17, 21]. All these methods use the measurement of the local ion conductance to generate images of sample topography. For many applications, however, it becomes important to measure complementary quantities, most prominently such that allow a determination of sample topography independent of the ion current. For this purpose, two different techniques have been developed so far: (a) SICM with a complementary AFM distance control [12] and (b) SICM with a complementary shear-force control [15]. The first technique uses a bent nanopipette that is coated with a reflective metal layer and that is scanned over the sample surface like an AFM tip. Different AFM imaging modes can be used this way, including contact mode and tapping mode imaging. The second technique uses a nanopipette that is positioned perpendicularly to the sample surface and that is set into transverse vibrations. Arising mechanical shear-forces between tip and sample provide an independent measure of sample height. Both techniques allow the simultaneous and complementary imaging of sample topography and local ion conductance. We organize this chapter in the following way: in Sect. 3.2, we cover fundamental principles concerning the measurement of the local ion conductance. In Sect. 3.3, we present theoretical approaches and experimental implementations for measuring ion currents through nanopipettes close to surfaces. In Sect. 3.4, we move on to advanced techniques for the imaging of ion currents that are based on the local measurement of conductance only. In Sect. 3.5, we finally move our attention to the combination of SICM with other scanning techniques. Methods that provide an independent measurement of sample topography are especially important as they enable high-resolution measurements of the local permeability of a sample to ions.
3.2 Fundamental Principles 3.2.1 Basic Setup The basic principle of SICM is shown in Fig. 3.1a. A nanopipette with a small opening diameter is positioned close to a sample surface. A voltage is applied accross the electrolyte via two electrodes, one inside the pipette and the other one in the bath
3 Scanning Ion Conductance Microscopy
93
Fig. 3.1. (a) Schematic of a basic SICM setup for current measurements over a non-porous sample. The tip of a pulled nanopipette is brought into close proximity to the sample surface. A voltage, U, is applied between the electrode in the pipette and that in the bath, causing an ionic current to flow through the opening of the pipette tip. With decreasing tip-sample distance, this current decreases as a result of the “squeezing” of the current into a narrowing conductance path (gap) between pipette and sample. Since no mechanical contact occurs during this process until “touch-down”, the measured leakage current, IL , provides a contact-free measure of tip-sample distance. By scanning the sample with respect to the pipette tip, two-dimensional images of sample topography can be recorded. (b) Equivalent circuit for this setup. The resistance of the pipette, RP , is in series with the resistance of the leakage path, RL
solution. Usually, silver/silver chloride electrodes are used. The induced current flows from the pipette electrode through the pipette, leaves the pipette through the narrow gap between pipette and sample surface, and is collected by the bath electrode (the direction of the current can also be reversed). The closer the pipette tip is to the sample, the more this leakage current is restricted (“squeezed”) by this narrow gap [9,22]. The detected current therefore directly gives a measure of the tip-sample distance. Especially important is the fact that this measurement is achieved without actual mechanical contact between tip and sample. It is therefore possible to record non-contact images of sample topography by scanning the sample relative to the tip and by using a feedback loop for controlling the tip-sample distance. We will see below that this property is especially valuable for the imaging of soft biological samples such as living cells. To further characterize this basic SICM measurement setup, we consider the equivalent circuit (Fig. 3.1b). The applied voltage, U, drives a current between the electrodes. This current needs to pass through the narrow neck of the pipette tip that constitutes the resistance RP , and, in series, through the leakage resistance of the thin gap between pipette and sample, RL . Since it is this leakage resistance that is usually of interest as it provides a measure of the tip-sample distance, it must not be much smaller than the pipette resistance. Otherwise, the overall resistance and therefore the measured current, I, would be dominated by the pipette resistance. This makes it difficult to extract the leakage resistance which becomes increasingly
94
T.E. Schäffer · B. Anczykowski · H. Fuchs
larger for smaller tip-sample distances. We assume here that other resistances in the system such as resistances in the wires, in the bulk electrolyte and in the solid-liquid junctions are small. Furthermore, we neglect electrochemically induced potentials that can be compensated for by applying an offset voltage. We also note that, when fast changes of the current are to be measured, the capacitances in the system need to be considered. In many cases it will be interesting to measure the current through conductive paths in the sample, such as pores or channels. For this purpose, we consider a slightly different setup (Fig. 3.2a). Characteristic for this type of measurement is that there is a separate compartment on each side of the sample. Each compartment is filled with electrolyte, and there are one or more conductive paths through the sample between the two compartments. Similarly to the setup described in Fig. 3.1, the thin end of a pulled pipette is brought into close proximity to the sample surface. One electrode is inside the pipette, and the other electrode is in the compartment below the sample. Again, a voltage is applied between the electrodes. Now there are different paths for the current. If the pipette would form an ideal, tight seal with the sample, then the only possibility for the current would be to travel through a conductive path (pore or channel) in the sample directly below the tip (IC ). In a realistic case, however, the seal is never perfect. Some current “escapes” through the thin gap between pipette and sample, and subsequently flows through the sample via other conductive paths, making up the leakage current, IL , that acts as a background current.
Fig. 3.2. (a) Schematic of a basic SICM setup for current measurements through a porous sample. There are two separate compartments with the sample at their interface. The pipette with the pipette electrode is placed above the sample, and the bath electrode is placed below the sample. The current can leave the pipette opening either through a conductive path in the sample directly below the tip (IC ) or can “escape” sideways through the thin gap between tip and sample as leakage current, IL . The closer the tip is to the sample surface, the smaller this leakage current is (due to the current squeezing effect), and the better the conductance through the sample can be measured. (b) Equivalent circuit for this setup. The resistance of the conductive path through the pore directly below the tip, RC , and the resistance of the leakage path, RL , are in parallel with respect to each other, and in series to the pipette resistance, RP
3 Scanning Ion Conductance Microscopy
95
We again consider the equivalent circuit to further characterize this setup (Fig. 3.2b). The current first passes through the narrow neck of the pipette tip that constitutes the resistance RP . The following two paths are symbolized by the channel resistance, RC , and by the leakage resistance, RL , in parallel to each other. Since we are usually interested in the current IC that flows through the channel below the tip, we need to measure RC . Therefore, the pipette resistance RP should be as small as possible, and the leakage resistance RL should be as large as possible, requiring the gap between pipette and sample to be small. 3.2.2 Nanopipettes Pipettes for SICM face similar requirements as those used for intracellular recording. Most importantly, they need to be quite sharp at the tip, with opening diameters of a few tens of nanometers. This minimizes the risk of cell damage during cell puncturing in intracellular recording, and maximizes the resolution in SICM. Pipettes are usually drawn from glass (e.g., borosilicate) capillaries with an initial outer diameter of 1–2 mm. Pipette pullers based on a heated coil can be used, but laserbased pipette pullers are preferable. In these pipette pullers an infrared laser beam locally heats up the glass capillary which is subsequently drawn apart by force. This creates sharp tips with opening diameters down to a few tens of nanometers (Fig. 3.3). A small opening diameter results in a relatively large pipette resistance RP . To minimize this resistance, the pipette could be filled with a highly conductive solution (e.g., 2–3 M KCl). The diffusion of this solution into the bath solution
Fig. 3.3. Scanning electron microscope (SEM) image of the tapered end of a nanopipette as it is typically used as an SICM probe (sputter coated with a thin layer of platinum to improve SEM imaging). The size of the opening depends on the pulling parameters such as pulling force, velocity, and heat. Inner opening diameters in the range of 30–100 nm are routinely obtained
T.E. Schäffer · B. Anczykowski · H. Fuchs
96
would be small due to the small tip diameter, and could be further reduced with the help of an agar salt bridge, for example. Physiological electrolyte solution of lower concentration, however, also works, resulting in typical pipette resistances on the order of 100 MΩ. 3.2.3 Electrodes The electrodes that are typically used in SICM are silver/silver chloride electrodes. This type of electrode is also used as reference electrodes in potentiometry and voltammetry experiments. Silver/silver chloride electrodes have electrochemical properties that make them well suited for application in SICM. Furthermore, they are easily fabricated, for example by electrolytic deposition of silver chloride on a layer of metallic silver. The silver/silver chloride (Ag/AgCl) electrode consists of a silver (Ag) wire that is coated with solid silver chloride (AgCl) and immersed in an electrolyte containing chloride ions (e.g., a solution of KCl or NaCl). In thermodynamic equilibrium, the solution is saturated with silver chloride: AgCl(solid) Ag+ (aq) + Cl− (aq)
(3.1)
The equilibrium constant for this reaction is K = 1.76 × 10−10 (T = 25 ◦ C), so the concentration of Ag+ ions in solution is very small. The Ag/AgCl electrode is described by a reversible redox reaction, in which the chloride atoms in the solid silver chloride receive an electron and go into solution as chloride ions, leaving metallic silver, and vice versa: AgCl(solid) + e− Ag(solid) + Cl− (aq)
(3.2)
This reaction occurs close to the electrode surface (< 1 nm distance). The potential that will build up at the electrode in thermodynamic equilibrium is given by the Nernst equation. The Nernst equation relates the electrode potential, E, to the concentration (more precisely: the activity) of the chloride ions in solution [23]. RT 1 ln F [Cl− ] ∼ = +0.222 V − 0.0591 V × lg[Cl− ]
E = E0 +
(3.3)
E 0 is the standard potential of the Ag/AgCl electrode (with respect to the Standard Hydrogen Electrode, at T = 25 ◦ C), R ∼ = 8.315 J mol−1 K−1 is the molar gas constant, T is the absolute temperature (here: T = 298 K), F ∼ = 96,485 C mol−1 is the Faraday constant, and the square brackets denote the concentration. In SICM, two Ag/AgCl electrodes are used as anode and cathode, respectively. This setup is simpler than that for voltammetric experiments, where three electrodes (working electrode, auxiliary electrode and reference electrode) are used and controlled by a potentiostat. For the SICM setup, simply an external voltage is applied between the two electrodes inducing a faradaic ionic current in the electrolyte which is measured with a low-current amplifier.
3 Scanning Ion Conductance Microscopy
97
3.3 Ion Currents Through Nanopipettes 3.3.1 Background Theory The measured current, I, that passes through the pipette depends on the effective ohmic resistance in the current path of the electrolyte, Reff : I=
U . Reff
(3.4)
U is the applied voltage. The resistance of the electrolyte is mainly determined by the narrow regions it passes through. Considering the equivalent circuit of Fig. 3.2b, the effective resistance becomes Reff = RP +
RC RL . RC + RL
(3.5)
We are often interested in the channel resistance RC . However, the channel resistance depends on the particular configuration in which it is measured. For configurations with simple boundary conditions, the channel resistance can easily be calculated. For example, for a cylindrical channel of length L and radius r that is capped by a (perfectly conducting) electrode at each opening, the ohmic channel resistance is given by capped
RC
=
Lρ , πr 2
(3.6)
where ρ is the specific electrical resistivity of the electrolyte. Such an ideal configuration, however, never occurs in SICM. A more realistic configuration is when the electrodes are far removed from either end of the conductive channel. The resistance then increases, because the current additionally traverses the distance from the bulk medium to the disk-like mouths of the channel. This gives rise to an “access” ∞ that acts in series with the channel resistance [18]: resistance Racc & πr ' ρ capped ∞ + Racc = L+ . (3.7) RC∞ ≈ RC 2 πr 2 But also this configuration does not precisely apply to SICM, mainly because one electrode is always confined to the interior of the pipette. The precise meaning of RP , RC and RL in (3.5) therefore depends on the particular boundary conditions (for example, the tip-sample distance). Nevertheless, (3.5) is useful in many cases, since it provides a simple allocation of the resistances in the current path. 3.3.2 Simple Analytical Model At the heart of SICM lies the dependence of the measured current on the tipsample distance that comes about in so-called current-distance curves. Far away
T.E. Schäffer · B. Anczykowski · H. Fuchs
98
from the sample surface, the current through the pipette is determined by the pipette resistance RP . Speaking in terms of (3.5), the leakage resistance is zero. In closer proximity to the sample surface, the leakage resistance increases due to the current squeezing effect. Therefore, the effective resistance increases and the measured current drops. In the ideal case of a perfect seal between pipette and surface at zero tip-sample distance, the current becomes zero at contact. In the case of a conically tapered pipette tip with an opening angle that is not too large, the pipette resistance can be approximated by [15] RP ≈
ρ LP , πr0 ri
(3.8)
where r0 is the inner diameter of the thick end, ri is the inner diameter of the thin end (at the pipette tip), and L P is the length of the conical pipette (Fig. 3.4, inset). This formula can be derived by sectioning the cone into successive disks of infinitesimal thickness, and summing the resistances of all disks (this assumes that disk-shaped electrodes are placed in the openings of the thin and the thick end). Nitz et al. [15] constructed a simple analytical model for the distance-dependent leakage resistance RL (in the absence of channels in the sample, i.e. RC → ∞). They obtained RL (z) ≈
3ρ ln(ra /ri ) , 2πz
(3.9)
where ra is the outer diameter of the thin end (pipette tip) and z is the tip-sample distance. The measured current thus becomes & z 0 '−1 I(z) ≈ I0 1 + , (3.10) z where I0 = U/RP is the measured current in the absence of the sample (or with a large tip-sample distance) and z0 =
3r0 ri ra ln . 2L P ri
Fig. 3.4. Calculated current vs. distance (IZ) curve, based on a simple analytical model [inset and (3.10)]. The parameters used for calculating the curve are r0 = 0.3 mm, ri = 50 nm, ra = 85 nm, L P = 10 mm, ρ = 1.09 Ω m and U = 100 mV
(3.11)
3 Scanning Ion Conductance Microscopy
99
Equation (3.10) describes a current that drops to zero for z = 0 and that asymptotically approaches I0 for z → ∞. At z = z 0 , the current is half of that asymptotic value. For typical parameters (r0 = 0.3 mm, ri = 50 nm, ra = 85 nm, L P = 10 mm, ρ = 1.09 Ω m, U = 100 mV), we obtain I0 = 432 pA and z 0 = 0.52 nm. It becomes apparent that the current starts to significantly drop only at very small tip-sample distances (Fig. 3.4). 3.3.3 Finite Element Modeling In order to further characterize and understand current flow when the pipette tip is close to a sample, we modeled the system using finite elements [24]. Due to the numerical nature of this modeling, more complex configurations can be analyzed. For example, it becomes straightforward to include a channel in the sample. We chose a conical pipette with an inner and outer tip opening diameter of 100 nm and 200 nm, respectively, and with an inner opening half-angle of 6◦ . We placed the pipette electrode in the plane 1000 nm into the pipette, and the bath electrode in the plane 320 nm below the tip opening. A cylindrical sample disk with a diameter and thickness of 700 nm and 30 nm, respectively, was placed concentrically below the pipette. Optionally, a thin concentric channel of 40 nm diameter was inserted in this sample disk. The electrolyte was assumed to be a 0.1 M NaCl solution, with a specific electrical resistivity of ρ = 1.09 Ω m [25]. The pipette walls and the sample were assumed electrical insulators. The governing differential equation of this system is the Poisson equation for the scalar electrical potential φ, ∆φ = 0 ,
(3.12)
where ∆ is the Laplace operator. The problem was then solved self-consistently with finite element modeling. Dirichlet boundary conditions apply at the pipette and bath electrodes, between which the voltage of 0.1 V was applied. Homogenous Neumann boundary conditions apply at the pipette walls and the sample, as well as at the system boundaries. The dimensionality of the system in the modeling process was reduced from three to two spatial dimensions by utilizing the cylindrical symmetry. The current density vector j directly derives from the electric field vector E, which in turn directly derives from the scalar electric potential: j=
1 1 E = − ∇φ . ρ ρ
(3.13)
The current flowing through the pipette was then simply obtained by integrating the current density over an area A spanning fully across the pipette interior, where only components of the current density that are normal to the local area element were considered: j · dA .
I=
(3.14)
A
The dot denotes the scalar product. We modeled three different experimental configurations. First, we removed the sample from the system, leaving only the pipette
100
T.E. Schäffer · B. Anczykowski · H. Fuchs
in the bath solution. The results of the finite element modeling process for this configuration are displayed in Fig. 3.5a. The local current density vectors in the axial symmetry plane are symbolized as arrows. Additionally, the absolute value of the current density is encoded in the grayscale, where darker areas denote larger current densities. It is apparent that the current density inside the pipette close to its tip is large (∼ = 1 − 2 × 105 A/m2 ), and that it drops to almost zero soon after leaving the pipette opening (within a distance of about half of the tip opening diameter). The total current flowing through the pipette is ∼ = 1.41 nA (corresponding to Reff ∼ = 70.9 MΩ). In Fig. 3.5b, we consider a different configuration by positioning an insulating sample surface 20 nm away from the pipette tip. This case demonstrates the current squeezing effect, as the current now has to escape sideways through the narrow gap between pipette tip and sample surface. But this relatively small tip-sample distance (20% of the tip diameter) does not lower the total current through the pipette (∼ = 77.5 MΩ) = 1.29 nA, corresponding to Reff ∼ by a large amount, compared to the case in Fig. 3.5a. This behavior will be discussed more below. In Fig. 3.5c, we add a small concentric channel with a diameter of 40 nm to the sample. Some of the current can now escape through this channel, thereby decreasing the effective resistance of the system. The total current through the pipette increases again slightly to ∼ = 1.33 nA (corresponding to Reff ∼ = 75.2 MΩ). It becomes apparent that even at these relatively small tip-sample distances, the influence of the sample, with or without channels, is relatively small. For larger effects to occur, the pipette tip needs to be positioned even closer to the sample, as we will see in the following paragraph. We repeated these modeling steps for a series of tip-sample distances, and plotted the total current as a function of tip-sample distance (Fig. 3.6). In the absence of the conductive channel through the sample (dashed line), the current starts to drop significantly at tip-sample distances below 20 nm (about half of the tip radius). At zero distance, the current is zero. In the presence of the conductive channel (solid
Fig. 3.5. Finite element analysis of the current squeezing effect at the tip of the pipette. (a) Pipette tip in the absence of a sample. The current density is large inside the pipette close to its end, and drops to almost zero soon below the pipette tip. (b) Pipette tip in the presence of a solid insulating sample. This added constraint causes the current to “leak” through the gap between tip and sample. (c) Pipette tip in the presence of a sample with a concentric channel below the tip. The current takes two alternative paths: it “leaks” through the gap between the tip and sample, and it flows through the channel in the sample. With a decreasing tip-sample distance, an increasing amount of current flows through the channel in the sample. For all three images, the arrows symbolize local current density vectors and the grayscale quantizes the absolute value of the current density. The parameters of the model are listed in the main text. Grayscale range (white to black): 0 − 2 × 105 A/m2
3 Scanning Ion Conductance Microscopy
101
Fig. 3.6. Calculated current vs. distance (IZ) curve, based on a finite element analysis. Two cases are considered: a sample without a central conductive channel (dashed line) and a sample with a central conductive channel (solid line). In both cases, the current starts to drop significantly only at tip-sample distances below half of the pipette tip radius. In the presence of the channel, the current reaches a finite value at zero distance, while it drops to zero in the absence of the channel
line), the current behaves similarly, but does not drop below a minimum value (here: ≈ 0.95 nA). In this case, the leakage current is zero and all the current flows through the channel in the sample. 3.3.4 Experimental Current-Distance Curves Current-distance curves manifest the basic principles of SICM, and provide useful information about the tip-sample interaction. In experimental current-distance curves, the pipette tip is ramped towards the sample surface with the help of a piezoelectric actuator (in z-direction). Simultaneously, the pipette current is recorded. A typical curve is shown in Fig. 3.7. When the pipette tip is far away from the sample surface, the current is about constant and independent of the z-piezo position (right hand side of graph). When the tip-sample distance gets in the range of the opening radius of the pipette tip, the cross section of the current path will decrease due to the thin gap forming. The resistance therefore increases and the measured current decreases. In
Fig. 3.7. Measured current vs. distance (IZ) curve on a glass surface. The current significantly decreases from a constant value to almost zero when approaching the surface. The inner tip radius of the pipette was 150 nm [15]
102
T.E. Schäffer · B. Anczykowski · H. Fuchs
the case of soft samples, often there is a seal that forms between the tip and sample, causing the measured current to decrease to almost zero. This is in contrast to hard samples such as glass coverslips, where the current often does not reach zero at any tip-sample distance. The reason for this is that neither the tip nor the sample is deformable to even out a slightly tilted or rough pipette opening, so a gap of finite size will be maintained. In many cases, the current starts to increase again when the pipette is further lowered into the sample. This effect has been attributed to a bending of the pipette that increases the leakage current [15]. 3.3.5 Imaging with Ion Current Feedback The dependence of the measured ion current on the tip-sample distance can be utilized to control this distance. This allows scanning the tip laterally over a sample at a preset vertical distance. Generally, scanning is achieved with the help of piezoelectric actuators that move the tip relative to the sample in each of the three spatial dimensions. A feedback loop keeps the tip-sample distance constant by controlling the vertical piezoelectric actuator so that the measured ion current stays constant. Simultaneous scanning in lateral direction then generates a topographic image of the sample surface (Fig. 3.8). One characteristic of this ion current feedback is that topographic data is obtained without mechanical contact between tip and sample. Gentle imaging of very soft samples such as living cells is therefore possible. Korchev et al., for example, imaged the topography of living cells with SICM to monitor dynamic changes in cell volume at a resolution of 2.5 × 10−20 liter [26] and to localize single active ion channels on the cell surface [27]. The lateral resolution of SICM topography images, however, is typically limited to several dozen nanometers, set by the inner opening diameter of the pipette tip. In the next section, we will discuss improvements of the current feedback technique that allow an even better and more reliable tracking of the sample surface.
Fig. 3.8. Topography of a monolayer of MDCK cells on a glass support, imaged with SICM in ion current feedback. Vertical range: 8.2 µm. Image size: 26.4 × 26.4 µm2 . Experimental data by P. Heidenreich, University of Münster
3 Scanning Ion Conductance Microscopy
103
3.4 Advanced Techniques The original SICM technique utilized the distance-dependence of the ion current to control the tip-sample distance with the help of a feedback loop. Provided that no local or temporal variations in the conductivity of the electrolyte occur, the feedbackcontrolled scanner will keep the distance between the probe and the sample constant while scanning the surface. Although this approach has successfully been applied to image the topography even of delicate biological samples, some inherent issues and weak points remain. Some of the problems of the original SICM setup will be discussed in the following paragraph. Since the SICM relies on a measurement of the dc ion current flowing between the pipette and the bath electrode, its performance strongly depends on the long-time stability of the overall electrochemical conditions. Various factors can affect in particular the dc voltage and current between the electrodes. For instance, temperature drifts as they can easily occur during scanning for hours can cause significant dc offsets, which in turn have a direct effect on the current-based feedback system. Furthermore, drifts due to a gradual contamination of the electrodes over time can also degrade the performance of the scanning system, ultimately making it impossible to track the sample topography for a long time. If the SICM is to be combined with other electrophysiological investigations further problems may arise. For instance the application of drugs or additional voltages or currents can also have significant effects on the electrochemical potential between the SICM electrodes. Using the dc ion current as a feedback signal might therefore be impractical. Another inherent weak point of a current-based feedback system results from the geometric shape of the pipette’s tapered end. In order to obtain a significant current squeezing effect when the probe is brought into close proximity to the sample surface, the tapered end should be even and flat. Such a leveled probe typically shows a strong dependency of the ion current on the vertical tip-sample distance. At the same time, however, this geometry makes the probe practically insensitive to protrusions on the sample surface if they are approached from the side during lateral scanning. As a consequence, the probe runs into these protrusions and then bends due to the lateral movement of the scanner. Such a bending will result in a small tilt of the opening of the pipette with respect to the sample surface, leading to a reduction of the squeezing effect and thereby to an increase of the ion current. The feedback loop of the SICM will then force the probe even further toward the sample, ultimately causing a tip crash and damaging both sample and probe. For the same geometric reasons the probe can easily get trapped in pits or pores that might be present on the sample surface. In general, rough surface morphologies are therefore difficult to scan in a stable manner with a simple current-based feedback system. As a first remedy the average distance between the probe and the sample could be kept rather large by simply adjusting the current setpoint of the feedback loop accordingly. Such a workaround, however, would degrade the sensitivity and the resolution of the SICM. Therefore, advanced techniques are required to overcome the inherent technical limitations of a simple current-based feedback system. A number of different approaches have been conceived to achieve this goal. They can be subdivided into two classes: SICM systems of the first class still rely on using the
104
T.E. Schäffer · B. Anczykowski · H. Fuchs
ion current as feedback signal for distance control, but apply special modulation techniques to minimize effects of the afore mentioned issues. We will discuss those techniques in the following paragraphs. In the second class of advanced SICM systems, the original concept of a current-based feedback system is abandoned. Instead, the SICM is provided with a current-independent feedback system to control the tip-sample distance. The local ion current is no longer used for distance control but recorded simultaneously with the surface topography as it is measured by a separate feedback system. Typical implementations are based on concepts well-known from other scanning probe techniques such as dynamic mode atomic force microscopy or shear force concepts. We will discuss them in detail in Sect. 3.5. 3.4.1 Modulation Methods Different methods for improving the performance of an SICM while retaining the original idea of using the local ion current as feedback signal for controlling the tip-sample distance have been introduced. In particular, modulation techniques have proved to be effective for minimizing the inherent problems of a current-based feedback loop. They share the common idea that the risk of hitting a surface feature during lateral scanning can be effectively reduced by modulating the tip-sample distance. Furthermore, modulation techniques can be useful to overcome limitations of the original SICM concept regarding long-term stability as they are caused by dc offsets and drift effects. Gitter et al. [28], Mann et al. [29] and Happel et al. [30] employ a type of pointspectroscopy technique as it is know from other scanning probe methods such as atomic force microscopy [31]. Here the probe is approached to and then retracted from the sample surface by typically several micrometers in each data point of the scanning area. Thus the lateral movement of the scanner can be performed while the probe is far away from the surface. Consequently, the risk of the probe laterally colliding with a protrusion on the surface or it getting trapped in a depression is reduced. However, this comes at the price of slow scanning speed, since the probe is not tracking the surface under continuous control of a feedback loop. Instead in each data point the probe is approached toward the sample until a predefined trigger point is reached, i.e. until a decrease of the ion current below a set threshold value signals that the probe is in close proximity to the surface. The z-position of this trigger point is stored and then the vertical movement is reversed and the probe retracted from the surface. This type of point-spectroscopy can practically be based on any type of trigger signal, for instance the “squeezing” effect of the dc ion current as it occurs typically a few tens of nanometers above the surface. While the point-spectroscopy approach provides an effective workaround for overcoming the inherently low lateral sensitivity of the probe, it does not address problems caused by time-varying dc offsets. To minimize such long term drift effects additional measures have to be taken. One option is applying either short voltage or current pulses [29, 30] instead of applying a constant voltage between the pipette and bath electrodes. This reduces unwanted effects caused by slowly changing dc potentials at the electrodes. Another method to improve the performance of a SICM with a current-based feedback
3 Scanning Ion Conductance Microscopy
105
Fig. 3.9. Setup of a distance-modulated SICM. The tapered pipette is attached to a piezo-electric element which modulates the distance between the probe and the sample surface. Typically a modulation frequency in the range of a few hundred Hertz and a modulation amplitude of a few tens of nanometers is applied. If the tapered end of the probe is in close proximity to the surface the resulting leakage current IL comprises a dc and an ac component. The amplitude of the latter depends on the average distance between the probe and the sample an serves as the input signal of a feedback loop
system has been proposed by the group of Shao [17, 21] and by the group of Korchev [16]. They keep the voltage between the two electrodes constant, but modulate the z-position of either the sample or the probe with an amplitude of a few tens of nanometers by means of a piezo-electric element (Fig. 3.9). If the probe is far away from the sample surface such a small distance modulation with a typical frequency of a few hundred Hertz does not significantly affect the ion current. If the tapered end of the pipette, however, is brought into close proximity to the surface so that the “squeezing effect” sets in, such a distance modulation leads to a modulation of the ion current. The amplitude of the resulting ac component in the ion current can then be detected with a lock-in amplifier. The latter allows recovering even noisy, low-level ion current signals by using the voltage signal which modulates the tip-sample distance as a reference signal. The detected amplitude of the modulated ion current is then used as feedback signal to control the average tip-sample distance, i.e. the feedback system tries to maintain a constant amplitude of the ion current while scanning the surface. This method of distance control has advantages over the conventional dc current-based approach because it makes the measurement less sensitive to changes in ionic strength or other dc drift effects.
106
T.E. Schäffer · B. Anczykowski · H. Fuchs
3.4.2 Applications in Bioscience Advanced modulation techniques as they were discussed in the previous section allow to scan delicate biological surfaces such as living cells more gently. The improved performance of a distance-modulated SICM allowed Gorelik et al. to obtain well resolved images of fine surface structures such as microvilli on living cells as depicted in Fig. 3.10 [32]. Since the introduction of the distance-modulation technique reduces the risk of uncontrolled contact between the probe and the sample and also improves long-term stability, it becomes possible to continuously image specific surface areas for several hours and thereby to study dynamic processes [33, 34].
Fig. 3.10. Monolayer of A6 epithelial cells imaged by distancemodulated SICM. The fine structure on the cell surface is well resolved and shows numerous microvilli. Reprinted with permission from Gorelik et al. [32]
Fig. 3.11. SICM scan of an A6 cell surface (left) and ion channel recording on top of a single microvillus (right). The pipette’s position is marked by an arrow in the line profile. The channel was identified as a K+ channel on the basis of the reversal potential of the current-voltage curve. Reprinted with permission from Gorelik et al. [32]
3 Scanning Ion Conductance Microscopy
107
Another type of application is to employ the SICM for performing patch-clamp experiments at specific surface sites [32, 34]. In such experiments the SICM is first used to scan the sample surface. The spatially resolved images of the surface topography allow identifying regions or structures of interest. The scan unit is then used to position the tapered SICM probe over a user-selected spot. Finally, the probe is engaged to the sample surface to form a gigaohm seal for subsequent patch-clamp recording. This combination of high-resolution SICM scanning and patch-clamping allows obtaining ion channel recordings on selective surface spots with lateral position control in the range of a few tens of nanometers. Such high precision is out of reach with conventional positioning methods such as those using light microscopy. With the SICM it becomes possible to investigate the activity of single ion-channels on nanometer-sized structures on native biological samples such as living cells. For instance, the tapered SICM pipette can be deliberately positioned on top of a single microvillus on an epithelial cell and used for subsequent patchclamp recording (Fig. 3.11).
3.5 Combination with Other Scanning Techniques The ability of the SICM to image biological samples in vivo with a resolution in the range of a few tens of nanometers makes it an interesting candidate for to combine with other scanning microscopy techniques. In doing so different strategies can be pursued: the first category of techniques sticks to the idea of using the ion current signal to maintain a constant distance between the probe and the sample while scanning. In addition a complementary data channel, for instance local optical data, is simultaneously recorded. Combinations of SICM with scanning nearfield optical microscopy (SNOM) or scanning confocal microscopy (SCM) fall in this category. The groups of Korchev and Shao modified the original SICM setup in such a way that the end of the tapered pipette also serves as a near-field light source for SNOM [21, 35, 36]. This can be achieved by coupling laser light into the pipette via an optical fiber. Coating the outside of the pipette with a reflective metal layer helps to confine the laser light to the aperture, i.e. the tapered pipette’s end. Provided that the sample and the substrate are transparent the SNOM signal can then be collected through an objective and detected by a photomultiplier located underneath the SICM head. Living cells were successfully investigated with such a combined SICM/SNOM setup by Korchev et al. An alternative way to utilize the SICM probe as a confined light source for SNOM was suggested by Bruckbauer et al. [37,38]. The method is based on fluorescence as it occurs when a calcium indicator, with which the pipette is filled, binds with calcium in the sample solution and is illuminated with a laser. The mixing zone where the fluorescent complex forms serves as a localized light source. SICM has also been successfully combined with SCM [39]. The setup comprises an inverted light microscope fully configured for scanning confocal microscopy, on which the SICM head is placed. During lateral scanning the vertical position of the sample is controlled by a standard SICM, i.e. ion current based feedback loop. As a consequence the optical confocal volume, which is located just below the pipette’s
108
T.E. Schäffer · B. Anczykowski · H. Fuchs
end, follows the topography of the sample. This allows capturing fluorescence images of a surface simultaneously with topographic data. Thereby interaction of fluorescent nanoparticles, for instance virus-like particles, with the surface of fixed or living cells can be studied. An alternative strategy for combining SICM with other scanning microscopy techniques abandons the original idea of an ion current based feedback system. Instead, other distance control schemes are employed to keep the scanned probe at a fixed, predefined distance to the sample surface and then to record local variations in the ion current as they might be caused by variations in local ion-conductivity or sample-permeability for instance. So far, we have considered only distance-control methods that are exclusively based on the measurement of the ion conductance. This works well for samples with a homogenous distribution of ion conductance. In many cases, however, it is of interest to study inhomogeneities in the local ion conductance, such as those that arise due to the presence of channels through a thin porous membrane, for example. In these cases, a mechanism independent from the ion conductance is required to keep the tip-sample distance constant. In the following sections we discuss different methods that solve this problem and present applications using these methods. 3.5.1 Combination with Atomic Force Microscopy One possibility for a simultaneous measurement of ion current and sample topography is based on the use of a bent nanopipette as a cantilever [12]. With such a configuration, the sample topography can be imaged using a standard AFM measurement setup. Simultaneously, the ion current can be monitored and recorded as a complementary measurement signal. The invention of the tapping mode in liquid [40, 41], which simplified imaging of soft samples in solution, initiated the development of a novel microscope: Tapping-mode AFM combined with a SICM [12]. In this design, a bent nanopipette [42, 43] is used as both force sensor and ion conductance probe (Fig. 3.12). This bent nanopipette is vibrated perpendicular to the sample with the help of a piezo stack. Typical vibration amplitudes at the tip are ≈ 10 nm rms. The measured vibration amplitude of the pipette serves as input signal to a feedback loop that controls the pipette-sample distance, thereby generating the topography signal when scanning. Simultaneously, the ion current is recorded and used to generate a complementary image of the ion conductance. While such a microscope can also be operated in contact mode (using the dc deflection of the pipette), better resolution (both in topography and ion conductance) is generally obtained in tapping mode due to the absence of lateral imaging forces. 3.5.2 Application in Material Science In this section, we will present an application of a tapping mode SICM in the field of biomineralization. This field deals with the processes by which living organisms synthesize organic-inorganic composite materials. These materials often exhibit elaborate micro- and nanostructures. They usually contain just a small
3 Scanning Ion Conductance Microscopy
109
Fig. 3.12. Combined scanning ion conductance microscope and tapping-mode atomic force microscope. A bent nanopipette is used as both an ion conductance probe and an atomic force microscope cantilever. Tapping mode operation enables topographic imaging of soft samples. The tip-sample distance is thereby kept constant by mechanically vibrating the pipette and using feedback to keep the vibration amplitude constant. The vibration amplitude of the cantilever is detected with nanometer precision using the optical beam deflection method. The pipette is coated with a layer of gold (thickness ≈ 30 nm) to increase its reflectivity. Simultaneously to the topography, the ion current through the pipette is recorded, thereby generating complementary images of topography and local ion conductance
amount of biopolymers, but those biopolymers play a critical role in the assembly of the mineral. Furthermore, these organic-inorganic composite materials often exhibit extraordinary mechanical, electrical, magnetic and chemical properties. By improving the knowledge about the mechanisms of biomineralization, new models might be created that aid in the artificial synthesis of new, high-performance materials. The example we will consider here is the formation of nacre (“mother of pearl”) by the marine mollusc Haliotis rufescens (red abalone). There has been a great interest in this material, and significant progress in the elucidation of its structure and function has been made over the last years. Nacre is a micro-laminate composite of highly oriented calcium carbonate (CaCO3 ) crystals in the aragonite polymorph and an organic matrix in the form of thin organic sheets, probably consisting of mostly proteins and polysaccharides. This composite material exhibits an intricate micro- and nanostructure of high regularity: it consists of an interdigitating brickwork array of crystal tablets and organic matrix. This composite structure is one of the reasons for the exceptionally large fracture toughness of nacre, which is ≈ 3000× larger than that of pure mineral. Various models have been set up that explain the fabrication process of nacre. With the use of electron diffraction microscopy and atomic force microscopy, it has
110
T.E. Schäffer · B. Anczykowski · H. Fuchs
Fig. 3.13. Schematic of a simple model of nacre growth, in which aragonite crystal tablets grow through pores in organic interlamellar sheets. SICM was used to proof the presence of such pores in the organic sheets, and to image their distribution and conductivity. (a) Side view. (b) Top view. Reprinted with permission from Schäffer et al. [13]. Copyright (1997) American Chemical Society
been found that the tablets are single crystals, and that the crystallographic axes of these crystals are nearly identical within several layers of subsequent tablets. This observation has resulted in a prominent model that explains the formation of nacre by a process called “hetero-epitaxial nucleation”. In this process, the growth of the crystal is periodically capped by an interlamellar organic layer, onto which a new crystal nucleates in a hetero-epitaxial fashion. Alternatively, abalone nacre may be formed by a continuous crystal growth of the mineral tablets through pores (channels) in the interlamellar organic sheets. Significant indirect and direct evidence has been favoring this alternate model that is based on growth through “mineral bridges” (Fig. 3.13). SICM was one of the techniques that generated strong evidence for this alternate model. For that purpose, demineralized interlamellar organic sheets were prepared from abalone nacre by decalcification. These organic sheets were imaged with a SICM in tapping mode operation without drying, fixing or coating the sample. The tapping mode operation ensured that a constant tip-sample distance was maintained. There are areas of high and low ion conductance on the organic sheet (Fig. 3.14a). In some areas with a predominantly low ion conductance, there are small features of locally enhanced ion conductance (Fig. 3.14b). With the help of a statistical analysis, these features were attributed to individual pores in the organic sheet. Several observations support this conclusion. First, the average ion conductance of these features is 28 ± 11 nS (after subtracting a conductivity background of 50 nS that is caused by leakage). From this quantity, the diameter of the pores in the organic sheet with a thickness of ≈ 30 nm calculates to 15–40 nm, which is in agreement with observations using atomic force or scanning electron microscopy. Second, an estimate of the pore density in the organic sheet can be found from the integrated conductance over the scan area. This estimate, 58 ± 12 pores/µm2 , is in the same range as the pore density seen in AFM images. Third, calcified features
3 Scanning Ion Conductance Microscopy
111
Fig. 3.14. SICM images of demineralized interlamellar organic sheets of abalone nacre. (a) Regions of small (dark) and large (bright) ion conductance can be seen, proving that the sheets are permeable for ions. Scalebar: 1 µm. Grayscale range (black to white): 50–200 nS. (b) Expansion of the box in (a). Some areas with predominantly low ion conductance show small, distinct features that might represent individual pores (arrows). Scalebar: 400 nm. Grayscale range (black to white): 50–200 nS. Reprinted with permission from Schäffer et al. [13]. Copyright (1997) American Chemical Society
that could be mineral bridges were observed using transmission electron microscopy (TEM). The realization that there are pores in the interlamellar organic sheets has several important consequences. On one hand, these pores can transport ions across those sheets, and possibly even soluble proteins that are necessary for growth control of the crystal tablets. But most importantly, there is the possibility that the crystal itself grows through those pores, thereby forming mineral bridges through the interlamellar organic sheets. This alternate model of nacre growth readily explains several experimental observations, among those the mentioned coherence of the crystallographic axes between consecutive tablets. 3.5.3 Combination with Shear Force Microscopy Another possibility for a simultaneous measurement of ion current and sample topography lies in the use of the nanopipette as shear force sensor. Shear force sensors are well known from SNOM setups, where they serve to keep an optical fiber at constant distance to the sample during scanning [44, 45]. In a shear force configuration, the nanopipette is vertically oriented with respect to the sample surface (Fig. 3.15). A small piezo-electric stack that is attached to the nanopipette excites transverse mechanical vibrations in the drawn-out end of the nanopipette (parallel to the sample surface). The vibration amplitude strongly depends on the tip-sample distance due to shear forces. The shear forces increase sharply at small tip-sample distances, thereby decreasing the vibration amplitude. The vibration amplitude is therefore well suited as a measure for the sample topography. The technical challenge is finding a method of detecting this vibration amplitude on the nanometer scale. Several methods have been established so far, including optical detection [44] and detection using a piezo-electric tuning fork sensor [46]. Piezo-electric detection
112
T.E. Schäffer · B. Anczykowski · H. Fuchs
Fig. 3.15. Schematic illustration of the setup of a combined scanning ion conductance and shear force microscope. The lateral oscillatory motion of the probe’s tapered end is induced by a piezo element to which the micropipette is attached. By focusing a laser beam on the tapered probe and detecting the diffracted light with a segmented photodiode the mechanical oscillation is converted into an electrical signal. This is analyzed by means of a lock-in amplifier whose reference channel is synchronized with the driving signal of the dither piezo. The amplitude of the probe’s oscillation serves as the input signal of a feedback loop. The latter controls the vertical position of the scanner in such a way that a constant, predefined oscillation amplitude is maintained during xy-scanning. As a consequence the SICM probe follows precisely the sample topography. Simultaneously the local ion current flowing between the electrodes in the micropipette and under the porous sample is recorded. Thus possible variations in the local ion conductivity can be analyzed along with the surface topography
methods face some principal problems when they are used for imaging in liquids, since electrical shortcuts may occur in the electrolyte medium. Solutions include coating the tuning fork with an electrical insulating layer [47], applying a custom piezo-electrical detection [48], or using a diving bell concept, where a water-air interface is forced close to the sample surface [49]. On the other hand, optical detection of shear forces principally works in liquid just as well as in air [50]. In the optical detection method, a laser beam is focused onto the vibrating section of the nanopipette near its tip (Fig. 3.15). The incident laser beam is scattered by the vibrating tip, thereby modulating the intensity distribution of the beam. An optoelectronic detector, usually based on a split photodiode, detects these intensity modulations of the scattered beam and generates a signal that is proportional to the vibration amplitude of the nanopipette. This signal is then fed to the scan controller that attempts to keep the signal constant with the help of a feedback loop, thereby generating a topographic image of the sample surface when scanning. Simultaneously, the ion current from an electrode below the sample to the electrode in the nanopipette is recorded and used to generate a complementary image of the ion conductance through the sample. One advantage of the shear force method over the tapping-mode method (Sect. 3.5.1) for measuring the tip-sample distance is that the pipettes need not go
3 Scanning Ion Conductance Microscopy
113
Fig. 3.16. Shear force topography image of a layer of fixed MDCK cells in buffer solution. Vertical range: 7.4 µm. Image size: 40 × 40 µm2 . Sample by S. Schrot, experimental data by M. Böcker, University of Münster
through the tricky process of being mechanically bent at their tip. One could think that the relatively large effective vertical spring constant of a vertically oriented pipette could impose a possible thread to soft samples. On the other hand, the non-contact nature of shear force imaging allows scanning of surfaces with small tip-sample interaction forces. It is possible to image soft samples as delicate as cells in liquid with a shear force setup (Fig. 3.16). The successful implementation of a combined scanning ion conductance and shear force microscope was demonstrated by Nitz et al. [15]. Using such a setup (Fig. 3.15), they acquired simultaneous images of topography and ion current on a polycarbonate membrane (Fig. 3.17). The locations of the pores can clearly be seen in the topography image as local depressions. The complementary ion current image shows an increased ion current at those locations. As further test samples, these researchers also used porous mica surfaces. Porous mica surfaces with defined pore sizes can be produced by a track-etching process [51]. In this process, a mica sample is irradiated with high energy ions, thereby inducing
Fig. 3.17. Complementary (a) shear force topography and (b) ion current images of a polycarbonate membrane with pores of 0.4 µm diameter. Image size: 6 × 6 µm2 . Reprinted with permission from Nitz et al. [15]
114
T.E. Schäffer · B. Anczykowski · H. Fuchs
Fig. 3.18. Complementary (a) shear force topography and (b) ion current images of a Muscovite mica surface in which rhombic pores with an opening area of 200×400 nm2 were inserted by ion radiation and subsequent etching with hydrofluoric acid. Image size: 3.2 × 3.2 µm2 . Reprinted with permission from Nitz et al. [15]
metastable states in the crystal lattice within a radius of 100 to 1000 nm from the ion trace. Subsequent etching with hydrofluoric acid produces rhombic pores with a diameter that can be influenced by the acid temperature and by the etching time. Simultaneous images of topography and ion current on such a porous mica surface show an increased ion current over the pores in the sample (Fig. 3.18), again demonstrating the feasibility of the shear force approach. 3.5.4 Application in Bioscience The combined scanning ion conductance and shear force microscope is an ideal tool for investigating local variations in the ion conductance of biological specimen. This is of special interest for research in the field of the barrier-forming structures such as endothelial or epithelial cell layers. In multicellular organisms such structures form the interface between different fluid compartments and play an important role for inter- and transcellular processes [52, 53]. Gaining insight into the complex barriercrossing transport mechanisms is a common interest of cell biology, medicine, and pharmacology, as malfunctioning of these barriers leads to pathological implications. In particular, knowledge about the permeability of barriers for substances such as drugs is of great relevance. Hence special electrochemical and microscopic methods are required to study the ion-permeability of barrier-forming cell structures. For instance, experimental techniques such as the measurement of transepithelial electrical resistances (TER) provide valuable information about the barrier properties of cell layers [54, 55]. In addition to such integrating measurements of the total cell layer impedance, the combined scanning ion conductance and shear force microscope can provide further insight into cellular transport mechanisms, because it allows the simultaneous recording of topographic data and local ion-conductance with high lateral resolution.
3 Scanning Ion Conductance Microscopy
115
Fig. 3.19. Complementary (a) shear-force topography and (b) ion current images of a layer of live MDCK-II cells. Some but not all of the cell-cell contacts are visible in topography. The simultaneously recorded current image shows an increased ion-permeability over tight-junctions, independent of the local surface corrugations. Image size: 22 × 22 µm2 . Sample provided by J. Seebach, experimental data by J. Kamp, University of Münster [66]
As depicted in Fig. 3.19, the shear-force-combined SICM has successfully been used to investigate intercellular structures, namely tight-junctions between living cells. The results show the benefits of having two independent information channels: while the topographic shear-force data alone does not permit to differentiate between a permeable ion-channel and a closed cavity in the cell layer, the ion current image provides this important piece of information. The possibility of this type of combined microscope to recognize ionic transport channels in hard as well as soft samples opens perspectives for further applications in fields as diverse as biochemistry/pharmacology, corrosion research, quality control of coatings or artificial membranes.
3.6 Outlook While the SICM itself already has a broad range of possible applications, further techniques which are based on similar components can be envisioned. For instance the tapered micropipette of the SICM can be used not only as a high-resolution scanning or patch-clamping probe for in vivo characterization of biological surfaces, but also as a source for localized material delivery. The material flux from the probe to the sample substrate can either be driven by electric fields, capillary forces, hydrostatic pressure, or by ultrasonic excitation. Such type of nanolithography has been successfully applied to deposit metals [56–59], chemicals [60, 61], and also biological material such as DNA, proteins or other biomolecules [62–65]. A possible field of application is the construction of nanostructured biosensors. Furthermore, having the ability to deliver material in a controlled manner through the micropipette of a SICM opens the perspective to study the effects of local drug delivery on
116
T.E. Schäffer · B. Anczykowski · H. Fuchs
biological specimen, providing a nanoscopic tool for drug-induced manipulation of individual cells. Acknowledgements. We thank M. Böcker, P. Heidenreich and J. Kamp for contributing to this chapter with their experimental results. We thank H.-J. Galla, A. Janshoff, M. Madeja, S. Schrot, M. Schwarz, J. Seebach, E.-J. Speckmann, C. Steinem, J. Wegener for support and discussions. This research was supported in part by the German Federal Ministry of Education and Research (BMBF), and by the Deutsche Forschungsgemeinschaft (DFG) by the Gemeinnützige HertieStiftung/Stifterverband für die Deutsche Wissenschaft (SCHA 1264).
References 1. Binnig G, Rohrer H (1982) Surface studies by scanning tunneling microscopy. Phys Rev Lett 49:57–61 2. Pohl DW, Denk W, Lanz M (1984) Optical stethoscopy: Image recording with resolution λ/20. Appl Phys Lett 44: 651–653 3. Binnig G, Quate CF, Gerber C (1986) Atomic force microscope. Phys Rev Lett 56:930–933 4. Drake B, Prater CB, Weisenhorn AL, Gould SA, Albrecht TR, Quate CF, Cannell DS, Hansma HG, Hansma PK (1989) Imaging crystals, polymers, and processes in water with the atomic force microscope. Science 243:1586–1589 5. Martin Y, Wickramasinge HK (1987) Magnetic imaging by “force microscopy” with ˚ resolution. Appl Phys Lett 50:1455–1457 1000 A 6. Sáenz JJ, García N, Grütter P, Meyer E, Heinzelmann H, Wiesendanger R, Rosenthaler L, Hidber HR, Güntherodt HJ (1987) Observation of magnetic forces by the atomic force microscope. J Appl Phys 62:4293–4295 7. Martin Y, Abraham DW, Wickramasinghe HK (1988) High-resolution capacitance measurement and potentiometry by force microscopy. Appl Phys Lett 52:1103–1105 8. Bard AJ, Fan F-RF, Kwak J, Lev O (1989) Scanning electrochemical microscopy. Introduction and principles. Anal Chem 61:132–138 9. Hansma PK, Drake B, Marti O, Gould SAC, Prater CB (1989) The scanning ionconductance microscope. Science 243:641–643 10. Prater CB, Drake B, Gould SAC, Hansma HG, Hansma PK (1990) Scanning ionconductance microscope and atomic force microscope. Scanning 12:50–52 11. Olin H (1994) Design of a scanning probe microscope. Meas Sci Technol 5:976–984 12. Proksch R, Lal R, Hansma PK, Morse D, Stucky G (1996) Imaging the Internal and External Pore Structure of Membranes in Fluid–Tapping mode Scanning Ion Conductance Microscopy. Biophys J 71:2155–2157 13. Schäffer TE, IonescuZanetti C, Proksch R, Fritz M, Walters DA, Almqvist N, Zaremba CM, Belcher AM, Smith BL, Stucky GD, Morse DE, Hansma PK (1997) Does abalone nacre form by heteroepitaxial nucleation or by growth through mineral bridges? Chem Mater 9:1731–1740 14. Korchev YE, Bashford CL, Milovanovic M, Vodyanoy I, Lab MJ (1997) Scanning ion conductance microscopy of living cells. Biophys J 73:653–658 15. Nitz H, Kamp J, Fuchs H (1998) A combined scanning ion-conductance and shear-force microscope. Probe Microsc 1:187–200 16. Shevchuk AI, Gorelik J, Harding SE, Lab MJ, Klenerman D, Korchev YE (2001) Simultaneous Measurement of Ca2+ and Cellular Dynamics: Combined Scanning Ion Conductance and Optical Microscopy to Study Contracting Cardiac Myocytes. Biophysical journal 81:1759–1764
3 Scanning Ion Conductance Microscopy
117
17. Pastré D, Iwamoto H, Liu J, Szabo G, Shao Z (2001) Characterization of AC mode scanning ion-conductance microscopy. Ultramicroscopy 90:13–19 18. Hille B (1992) Ionic Channels of Excitable Membranes, 2nd ed. Sinauer Associates, Sunderland, Mass. 19. Sakmann B, Neher E (1995) Single-Channel Recording, 2nd ed. Springer, Heidelberg 20. Prater CB, Hansma PK (1991) Improved scanning ion-conductance microscope using microfabricated probes. Rev Sci Instrum 62:2634–2638 21. Mannelquist A, Iwamoto H, Szabo G, Shao Z (2001) Near-field optical microscopy with a vibrating probe in aqueous solution. Appl Phys Lett 78:2076–2078 22. Bard AJ, Denuault G, Lee C, Mandler D, Wipf DO (1990) Scanning electrochemical microscopy: a new technique for the characterization and modification of surfaces. Acc Chem Res 23:357–363 23. Bockris JO, Reddy AKN (2000) Modern Electrochemistry: Electrodics in Chemistry, Engineering, Biology, and Environmental Science. Plenum Publishing Corporation, New York 24. QuickField SE. Tera Analysis Ltd., Svendborg, Denmark 25. Gehrtsen C, Kneser HO, Vogel H (1989) Physik, 16th ed. Springer, Berlin 26. Korchev YE, Gorelik J, Lab MJ, Sviderskaya EV, Johnston CL, Coombes CR, Vodyanoy I, Edwards CRW (2000) Cell Volume Measurement Using Scanning Ion Conductance Microscopy. Biophysical journal 78:451–457 27. Korchev YE, Negulyaev YA, Edwards CRW, Vodyanoy I, Lab MJ (2000) Functional localization of single active ion channels on the surface of a living cell. Nat Cell Biol 2:616–619 28. Gitter AH, Bertog M, J-DS, Fromm M (1997) Measurement of paracellular epithelial conductivity by conductance scanning. Eur J Physiol 434:830–840 29. Mann SA, Hoffmann G, Hengstenberg A, Schuhmann W, Dietzel ID (2002) Pulse-mode scanning ion conductance microscopy: A method to investigate cultured hippocampal cells. J Neurosci Methods 116:113–117 30. Happel P, Hoffmann G, Mann SA, Dietzel ID (2003) Monitoring cell movements and volume changes with pulse-mode scanning ion conductance microscopy. J Microsc 212:144– 151 31. Radmacher M, Cleveland JP, Fritz M, Hansma HG, Hansma PK (1994) Mapping interaction forces with the atomic force microscope. Biophysical Journal 66:2159–2165 32. Gorelik J, Yuchun, G., Spohr HA, Shevchuk AI, Lab MJ, Harding SE, Edwards CRW, Whitaker M, Moss GWJ, Benton DCH, Sanchez D, Darszon A, Vodyanoy I, Klenerman D, Korchev YE (2002) Ion channels in small cells and subcellular structures can be studied with a smart patch-clamp system. Biophys J 83:3296–3303 33. Gorelik J, Shevchuk AI, Frolenkov GI, Diakonov IA, Lab MJ, Kros CJ, Richardson GP, Vodyanoy I, Edwards CRW, Klenerman D, Korchev YE (2003) Dynamic assembly of surface structures in living cells. Proc Natl Acad Sci USA 100:5819–5822 34. Gorelik J, Zhang A, Shevchuk A, Frolenkov GI, Sanchez D, Lab MJ, Vodyanoy I, W ECR, Klenerman D, Korchev YE (2002) The use of scanning ion conductance microscopy to image A6 cells. Mol Cell Endocrinol 217:101–108 35. Korchev YE, Raval M, Lab MJ, Gorelik J, Edwards CRW, Rayment T, Klenerman D (2000) Hybrid Scanning Ion Conductance and Scanning Near-Field Optical Microscopy for the Study of Living Cells. Biophys J 78:2675–2679 36. Mannelquist A, Iwamoto H, Szabo G, Shao Z (2002) Near field optical microscopy in aqueous solution: implementation and characterization of a vibrating probe. J Microsc 205:53–60
118
T.E. Schäffer · B. Anczykowski · H. Fuchs
37. Bruckbauer A, Ying L, Rothery AM, Korchev YE, Klenerman D (2002) Characterization of a novel light source for simultaneous optical and scanning ion conductance microscopy. Analytical Chemistry 2002,74:2612–2616 38. Rothery AM, Gorelik J, Bruckbauer A, Yu W, Korchev YE, Klenerman D (2003) A novel light source for SICM–SNOM of living cells. J Microsc 209:94–101 39. Gorelik J, Shevchuk A, Ramalho M, Elliott M, Lei C, Higgins CF, Lab MJ, Klenerman D, Krauzewicz N, Korchev Y (2002) Scanning surface confocal microscopy for simultaneous topographical and fluorescence imaging – Application to single virus-like particle entry into a cell. Proc Natl Acad Sci USA 99:16018–16023 40. Hansma PK, Cleveland JP, Radmacher M, Walters DA, Hillner PE, Bezanilla M, Fritz M, Vie D, Hansma HG, Prater CB, Massie J, Fukunaga L, Gurley J, Elings V (1994) Tapping mode atomic force microscopy in liquids. Appl Phys Lett 64:1738–1740 41. Putman CAJ, Werf KOVd, Grooth BGD, Hulst NFV, Greve J (1994) Tapping mode atomic force microscopy in liquid. Appl Phys Lett 64:2454–2456 42. Shalom S, Lieberman K, Lewis A, Cohen SR (1992) A Micropipette Force Probe Suitable For Near-Field Scanning Optical Microscopy. Rev Sci Instrum 63:4061–4065 43. Lewis A, Taha H, Strinkovski A, Manevitch A, Khatchatouriants A, Dekhter R, Amman E (2003) Near-field optics: from subwavelength illumination to nanometric shadowing. Nat Biotechnol 21:1378–1386 44. Betzig E, Trautman JK, Harris TD, Weiner JS, Kostelak RL (1991) Breaking the diffraction barrier: optical microscopy on a nanometric scale. Science 5000:1468–1470 45. Toledo-Crow R, Yang PC, Chen Y, Vaez-Iravani M (1992) Near-field differential scanning optical microscope with atomic force regulation. Appl Phys Lett 60:2957–2959 46. Karraï K, Grober RD (1995) Piezoelectric tip-sample distance control for near field optical microscopes. Appl Phys Lett 14:1842–1844 47. Rensen WHJ, van Hulst NF, Kämmer SB (2000) Imaging soft samples in liquid with tuning fork based shear force microscopy. Appl Phys Lett 77: 1557–1559 48. Brunner R, Hering O, Marti O, Hollricher O (1997) Piezoelectrical shear-force control on soft biological samples in aqueous solution. Appl Phys Lett 71:3628–3630 49. Koopman M, de Bakker BI, Garcia-Parajo MF, van Hulst NF (2003) Shear force imaging of soft samples in liquid using a diving bell concept. Appl Phys Lett 83:5083–5085 50. Lambelet P, Pfeffer M, Sayah A, Marquis-Weible F (1998) Reduction of tip-sample interaction forces for scanning near-field optical microscopy in a liquid environment. Ultramicroscopy 71:117–121 51. Fischer BE, Spohr R (1983) Production and use of nuclear tracks: imprinting structure on solids. Rev Mod Phys 55:907–948 52. Powell DW (1981) Barrier function of epithelia. Am J Physiol 241: G275-G288 53. Simionescu M, Simionescu N (1986) Functions of the endothelial cell surface. Ann Rev Physiol 48:279–293 54. Wegner J, Zink S, Rösen P, Galla H-J (1999) Use of electrochemical impedance measurements to monitor ß-adrenergic stimulation of bovine aortic endothelial cells. Eur J Physiol 437:925–934 55. Wegner J, Abrams D, Willenbrink W, Galla H-J, Janshoff A (2004) Automated multi-well device to measure transepithelial electrical resistances under physiological conditions. Biotechniques 37:590–597 56. Zhang H, Wu L, Huang F (1999) Electrochemical microprocess by scanning ionconductance microscopy. J Vac Sci Technol B 17:269 57. Lewis A, Kheifetz Y, Shambrodt E, Radko A, Khatchatryan E, Sukenik C (1999) Fountain pen nanochemistry: Atomic force control of chrome etching. Appl Phys Lett 75:2689–2691 58. Müller A-D, Müller F, Hietschold M (1998) Electrochemical pattern formation in a scanning near-field optical microscope. Appl Phys A 66:S453–S456
3 Scanning Ion Conductance Microscopy
119
59. Müller A-D, Müller F, Hietschold M (2000) Localized electrochemical deposition of metals using micropipettes. Thin Solid Films 366:32–36 60. Hong M-H, Kim KH, Bae J, Jhe W (2000) Scanning nanolithography using a material-filled nanopipette. Appl Phys Lett 77:2604–2606 61. Larson BJ, Gillmor SD, Lagally MG (2003) Controlled deposition of picoliter amounts of fluid using an ultrasonically driven micropipette. Rev Sci Instrum 75:832–836 62. Ying L, Bruckbauer A, Rothery AM, Korchev YE, Klenerman D (2002) Programmable Delivery of DNA through a Nanopipet. Anal Chem 74:1380–1385 63. Bruckbauer A, Ying L, Rothery AM, Zhou D, Shevchuk AI, Abell C, Korchev YE, Klenerman D (2002) Writing with DNA and protein using a nanopipet for controlled delivery. J Am Chem Soc 124:8810–8811 64. Bruckbauer A, Zhou D, Ying L, Korchev YE, Abell C, Klenerman D (2003) Multicomponent Submicron Features of Biomolecules Created by Voltage Controlled Deposition from a Nanopipet. J Am Chem Soc 125:9834–9839 65. Taha H, Marks RS, Gheber LA, Rousso I, Newman J, Sukenik C, Lewis A (2003) Protein printing with an atomic force sensing nanofountainpen. Appl Phys Lett 83:1041–1043 66. Seebach J (2001) Einsatz elektrisch leitender Kultursubstrate zur Charakterisierung von Zell-Zell- und Zell-Substrat-Interaktionen, Dissertation thesis, University of Münster
4 Spin-Polarized Scanning Tunneling Microscopy Wulf Wulfhekel · Uta Schlickum · Jürgen Kirschner
Summary. We give an introduction to spin-polarized scanning tunneling microscopy (Sp-STM), a magnetic imaging technique with nanometer lateral resolution. Sp-STM allows to record constant current images which represent the electron density near the sample surface and simultaneously the spin polarization of the electron density which is related to the magnetic moment. It is shown how magnetic and topographic information can be separated using a modulation technique of the magnetization of bulk ferromagnetic tips. It is demonstrated that the out-ofplane component as well as one well-defined in-plane component of the spin polarization can be recorded. Finally, it is shown that with Sp-STM valuable information on the spin-resolved electronic structure and on the fundamental processes of tunneling spins may be obtained.
4.1 Introduction The imaging of magnetic domains in small structures is one of the important basis of modern micro-magnetism. While the existence of magnetic domains was initially not directly shown with an imaging technique, but was deduced from the observation of discontinuous jumps in the hysteresis loops [1], magnetic imaging has become the method of choice when investigating magnetic structures. Since the early works of Barkhausen, several magnetic imaging techniques, i.e. techniques that map one or more components of the magnetization or related quantities, were developed. The measured quantity can be e.g. the magnetic vector potential, the magnetization, the magnetic stray field or the spin polarization. We here focus on spin-polarized scanning tunneling microscopy (Sp-STM), which maps the spin polarization of a conductive sample surface. 4.1.1 The Resolution Problem in Magnetic Imaging In modern applications, e.g. magnetic recording media or magnetic random access memory, the size of the magnetic structures or domains is in the range of several 10 nm and the trend of miniaturization is still holding on. This poses some severe resolution problems to most established magnetic imaging techniques. For example, magnetic force microscopy (MFM) is intrinsically limited in lateral resolution by the physical effect used to obtain magnetic contrast. MFM relies on the long range magnetic dipolar interaction of a magnetic tip and the magnetic charges of the sample. To obtain reasonable forces, the magnetic volume of the tip has to be of sufficient
122
W. Wulfhekel · U. Schlickum · J. Kirschner
size. Further, the magnetic tip has to be lifted several nm above the surface to avoid other interactions like the van-der-Waals force to cover up the small magnetostatic forces. These constrains in localization of the interaction lead to a limit of the MFM resolution around several 10 nm [2]. Resolution limits of similar size exists for most other magnetic imaging techniques. More details on this can be found in [2]. To further develop new magnetic recording media, alternative magnetic imaging techniques are required. In fundamental studies of magnetism, there exists a similar need for high resolution magnetic imaging. Many fundamental questions in magnetism are linked to processes that operate on the atomic scale and are beyond the lateral resolution of the established techniques. At the forefront of nano-science, high resolution imaging techniques are in general of high interest and impact. Sp-STM may contribute substantially in the study of magnetism on the nanometer scale, as its resolution is given by the lateral extension of the tip area that contributes to the tunneling process. Under favorable conditions, this may lead to sub-nanometer lateral resolution [3, 4]. We illustrate the capabilities of this new technique and compare it to MFM. 4.1.2 Magnetism and Spin The key to Sp-STM lies in the relation of magnetism and the electronic structure of matter. In ferromagnets, the spin sensitive exchange interaction between localized electrons (Heisenberg model) or electrons in a delocalized electron gas (Stoner model) splits the electronic density of states into minority and majority densities (see Fig. 4.1a). This is in contrast to paramagnetic substances, where the distributions of spin-up and spin-down electrons are identical. In ferromagnets, the spin splitting leads to an imbalance of the total occupation of the electrons of different spins and as a consequence to the magnetic moment of the atom. The direction of magnetization of the ferromagnet is in general collinear to the direction of the spin polarization, which relates the magnetization to the spin polarization. A measurement of one or more of the components of the spin polarization can give information on one or more components of the direction of magnetization, respectively. 4.1.3 The Tunneling Magnetoresistance Effect The splitting of the density of states has immediate consequences on the tunneling current. Pioneering field-emission experiments with ferromagnetic tips have shown [5, 6] that during the tunneling process from the tip into the vacuum, the spin polarization of the density of states of the tip is partly transferred to the emitted electrons. A spin-polarized current was observed. This can easily be understood on the basis of Fermi’s golden rule. The tunneling process itself, i.e. the transmission probability through the potential step of the work function in front of the tip, is not spin dependent. The observed polarization is just a consequence of the different number of states for minority and majority electrons: the more states are allowed to tunnel, the higher the resulting tunneling current. In this simplified picture, the tun-
4 Spin-Polarized Scanning Tunneling Microscopy
123
neling current from a spin-polarized tip is spin-polarized according to the imbalance of electrons with spin-up and spin-down. Julli`ere discovered that when electrons tunnel between two ferromagnets, not only the current is spin-polarized but also the size of the current is influenced [7]. In his experiment, two magnetic films were separated by an insulator film to form a planar tunnel junction. The two magnetic films were chosen to have different coercive fields. This permitted to align their magnetization parallel or antiparallel as a function of an applied magnetic field. Julli`ere found that the tunneling conductance G (and by this the resistance) depends on the relative orientation of the magnetization of the two layers. This effect is called the tunneling magnetoresistance (TMR) effect. For parallel orientation G was higher than for antiparallel orientation. This finding can be explained on basis of a simple model. As above, we neglect any spin dependence in the transmission through the barrier and focus solely on the density of states of the two electrodes. Under the assumption of a small bias voltage across the junction and in the absence of spin-flip scattering, the density of states in the ferromagnets near the Fermi energy determine the tunneling conductance. For parallel orientation, the majority/minority electrons of the first electrode tunnel into the majority/minority states in the second electrode, respectively, as sketched in Fig. 4.1b. Using Fermi’s golden rule, the conductance G is proportional to the density N of initial (i) and final (f ) states at the Femi edge. Combining both spin channels, the conductance for parallel oriented magnetizations is given by: f
f
G ↑↑ ∝ N↑i N↑ + N↓i N↓
(4.1)
Fig. 4.1. (a) Spin-split density of states N of a ferromagnet. ↑/↓ indicate majority/minority states. (b), (c) Tunneling between two ferromagnetic electrodes. In (b) respectively (c) the magnetization of the two electrodes is parallel respectively antiparallel. The conductivities G for tunneling from the left to the right electrode are indicated by arrows
W. Wulfhekel · U. Schlickum · J. Kirschner
124
For antiparallel orientation (see Fig. 4.1c), electrons of majority character in one electrode tunnel into states of minority character in the other electrode and the conductance is given by a mixed product: f
f
G ↑↓ ∝ N↑i N↓ + N↓i N↑
(4.2)
These two conductivities in general differ leading to a variation of the tunneling current with the relative orientation of magnetization of the electrodes. Later, Slonczewski treated the problem of spin-polarized tunneling more rigorously [8]. Neglecting higher order spin effects like spin accumulation, he calculated the dependence of G on the angle θ between the magnetization of the two electrodes. With the spin polarization P = (N↑ − N↓ )/(N↑ + N↓ ), and neglecting barrier effects, the conductance is given by: G = G 0 (1 + P i P f cos θ)
(4.3)
Slonczewski’s calculations for the angular dependence of the TMR effect was later experimentally confirmed [9]. In general, if a finite bias is applied, all states between the two Fermi levels are involved in tunneling. They have to be weighted according to their tunneling probability, which is among other things energy dependent. This scenario is more complex but G can be expressed using effective, i.e. correctly weighted, densities or polarizations. More details on this will be given in Sect. 4.6.1.
4.2 The Principle of Spin-polarized Scanning Tunneling Microscopy With the invention of STM, Binning et al. realized an imaging technique with a lateral resolution that is capable to resolve single atoms [10, 11]. In STM, the apex of a conductive tip is placed near the surface of a conductive sample. Between sample and tip, a bias voltage is applied and a small tunneling current flows, that exponentially decays with tip sample separation. In the constant current mode of STM, a feed back mechanism adjusts the tip sample distance such that a constant tunneling current is obtained. When the tip is scanned over the surface, the tip apex moves on lines of constant current. In the simplest model, these lines are related to lines of constant density of states, i.e. reflect the sample topography. Already in 1988, Pierce suggested to set up a STM that uses the TMR effect to image simultaneously the sample magnetization [12]. All that is needed in addition to convential STM is a spin-polarized tunneling current. He suggested two different approaches to SpSTM. Besides the obvious use of ferromagnetic, i.e. spin polarized tips, he discussed the possibility to photo-excite spin-polarized carriers in GaAs tips. The latter was realized by Suzuki et al. [13]. In their approach, circularly polarized light was used to excite spin-polarized carriers into the conduction band of the tip that then tunnel into the sample. The spin polarization of the electrons can be selected by the helicity of the light. By modulating the helicity, modulations in the tunneling current were induced due to spin dependent tunneling. The modulations were detected with a lock-in amplifier to separate spin information from topographic information. The success of
4 Spin-Polarized Scanning Tunneling Microscopy
125
this approach was limited. It suffered from a rather low contrast and an unintended additional magneto-optical contrast of low lateral resolution. In this chapter, we focus on Sp-STM experiments with ferromagnetic tips. This approach was more successful. In the pioneering publication of Pierce, three different imaging modes of Sp-STM were suggested. All have been realized experimentally and are briefly explained below. We will, however, focus on only one of the three imaging modes. A detailed description of all imaging modes was given recently, elsewhere [14]. 4.2.1 The Constant Current Mode In the constant current mode, STM images are taken with non magnetic and ferromagnetic tips and the results are carefully compared. Wiesendanger et al. were the first to report results obtained with this mode [15] on the layer-wise antiferromagnetic Cr(001) surface [16]. Using tungsten tips, topographic constant current line-scans revealed atomic steps on Cr(001) of the expected step height of 0.14 nm while using a ferromagnetic CrO2 tip, alternating step heights of 0.16 and 0.12 nm were observed. This was attributed to the TMR effect between the ferromagnetic tip and the ferromagnetically ordered Cr atoms on the terraces. When the spin polarizations of the tip and the Cr terrace atoms are parallel, the tunneling current is enhanced due to the TMR effect (see (4.3)) and in the constant current mode of the STM, the tip is retracted by a small amount (0.02 nm). On the adjacent atomic terrace on Cr, the spin polarization of the terrace atoms is opposite due to the topological antiferromagnetic order of Cr(001) [16]. Therefore, on this terrace the TMR effect leads to a reduction of the current and the STM tip approaches slightly. This mechanism results in alternating step heights seen with a spin-polarized tip. However, no separation of topography and spin information could be obtained in this imaging mode and reference measurements had to be acquired with non-magnetic tips. 4.2.2 The Spectroscopic Mode The spectroscopic mode of Sp-STM allows under certain circumstances the separation of topographic information from spin information. This mode is also named spin-polarized scanning tunneling spectroscopy (Sp-STS). It was initially suggested by Pierce [12] and Stroscio et al. [17] and was first realized by Bode et al. [18]. It uses the fact that the spin polarization of the tunneling current is a function of the energy, i.e. the spin polarization of the states that contribute to tunneling depends on the sample bias. For example, when a finite negative sample bias U is applied between tip and sample, in principle the occupied sample states in the range of width U below the Fermi level of the sample contribute to the tunneling. In the tunneling process, the electrons tunnel into the unoccupied tip states of the range U above the Fermi level of the tip. The spin polarization of both, the tip and the sample states, contribute to the tunneling. Therefore the spin polarization of the tunneling current in general varies with sample bias. To illustrate the mode of operation, let us assume that the spin polarization increases with U. When the magnetic surface is
126
W. Wulfhekel · U. Schlickum · J. Kirschner
imaged, the topographic image contains both information on the electronic density and on the spin, as mentioned above. Any variations of the conductance G due to the TMR effect are compensated by changes in the tip sample distance. In Sp-STS, the feed back loop of the STM is switched of and U is increased. As a consequence, the tunneling current changes. As we have assumed a rising spin polarization, the tunneling current for parallel oriented tip and sample magnetization increases more than for antiparralel orientation. Pierce et al. suggested to vary U significantly. Nevertheless, the imaging mode also works for small modulation of U. In this case, the variations in the tunneling current are proportional to the differential conductance dI/dU. In the pioneering experiment by Bode et al., the observed peak height of the spin-split surface state of Gd(0001) in laterally resolved dI/dU spectra was used to obtain magnetic information [18]. The imaging mode is now widely used. It has the advantage that tips coated with a thin film of a ferromagnet or antiferromagnet can be used so that the magnetic stray field of the tips can be minimized or completely be avoided [19, 20]. The obvious disadvantage is that the dI/dU signal in Sp-STS only weakly depends on magnetism. It much stronger depends on general variations of the density of states caused by e.g. compositional, structural or morphological changes of the sample. A more detailed overview on this imaging mode can be found in [2]. 4.2.3 Differential Magnetic Imaging Mode In the differential magnetic imaging mode, a bulk ferromagnetic tip is used whose magnetization is modulated. Due to the TMR effect, these modulations lead to modulations of the tunneling current that are related to the spin polarization of the sample. The basic concept of this mode is directly related to (4.3). In the experiment, a magnetically bistable tip is used. The tip magnetization is periodically switched between the two stable configurations of opposite magnetization. This is equivalent to changing the sign of the spin polarization of the tip apex. In the experimental set-up, the magnetization of the tip is reversed by an alternating current through a small coil that is fixed to the tip. The frequency of the alternating current lies above the cut-off frequency of the feed back loop of the STM [21]. Thus, the feed back loop only detects the averaged tunneling current for the two spin polarizations (positive and negative) of the tip apex. As can easily be seen from (4.3), in the averaged tunneling current I = I0 all spin-dependent currents cancel out such that the constant current image contains no magnetic information. With a phasesensitive lock-in amplifier, the alternating part of the tunneling current ∆I is detected which is proportional to P i P f cos Θ. It contains all the spin information. This way, topographic and spin information are strictly separated and an image of the spin component along the magnetization axis of the tip can be recorded simultaneously with the topography [21]. The alternating magnetic field induced within the coil has to be large enough to fully reverse the magnetization of the tip. The alternating field, however, also creates induction currents in the tunneling loop. For this reason, in an experiment only soft magnetic materials may be used as tips. Moreover, magnetostriction of the tip during the reversal must be avoided. The early experiments of Johnson et al. suffered from large magnetostriction of the Ni tip, so that no stable magnetic or topographic imaging was possible [22].
4 Spin-Polarized Scanning Tunneling Microscopy
127
4.3 Experimental Set-up In our experiment, the magnetization of a ferromagnetic electrode is switched by applying a small alternating current to a coil wound around the electrode. The direction of magnetization of the STM electrode is mostly determined by its shape. For imaging the out-of-plane component of the spin polarization, a sharp and pointed tip is used [23]. This is schematically shown in Fig. 4.2a. The alternating magnetic field induced by the coil is large enough to fully reverse the magnetization of the tip. In the tip, the magnetization direction lies always along the tip axis due to the large shape anisotropy. Thus, at the tip apex where the tunneling occurs, the magnetization is perpendicular to the sample surface. To image an in-plane component of the sample spin polarization, a ring is used as a STM electrode [24] as schematically shown in Fig. 4.2b. The magnetic field of the coil switches the ring between the two stable circular magnetic configurations. At the bottom of the ring, the magnetization lies tangential to the ring, i.e., in the surface plane. By choosing the plane in which the ring is oriented, the magnetization direction of the ring is defined and thus the direction of the sensitivity in the surface plane for the measured spin signal is known. Figure 4.3 shows images of the STM electrodes experimental realization. STM tips for recording the out-of-plane componen of the spin polarization (see Fig. 4.3a) were prepared by electrochemical etching from thin CoFeSiB wires of 130 µm diameter. As etching agent, a dilute mixture of HCl and HF was used that was suspended by surface tension as a thin liquid membrane in a Pt ring during etching. The pH value was tuned such that the formation of silica from the Si in the amorphous wire was prevented. Using low etching currents of the order of 250 µA, pointed tips of cone angles typically between 8 and 15◦ were created (see bottom of Fig. 4.3a). Due to the large shape anisotropy, the tip magnetization is along the tip axis [25]. The magnetic tips were fixed in a non magnetic shaft around which the coil is wound. The chosen tip material offers extremely low coercivities in the range of 50 µT and negligible magnetostriction (smaller than 10−8 ). This ensures that during switching of the tip, magnetization, the magnetostriction in the created domain walls is small enough that virtually all mechanical vibrations are suppressed [25]. With detailed micromagnetic simulations of the tip switching process, the expected magnetostriction could be estimated to be below 10−14 m, i.e. is irrelevant in the experiment. For imaging one in-plane component of the spin polarization, ring shaped STM electrodes of the same CoFeSiB material were used [24]. Figure 4.3b shows an
Fig. 4.2. Schematic representation of Sp-STM electrodes for measuring (a) the out-of-plane component and (b) the in-plane component of the sample spin polarization
128
W. Wulfhekel · U. Schlickum · J. Kirschner
Fig. 4.3. Sp-STM electrodes for measuring (a) the out-of-plane component and (b) the inplane component of the sample spin polarization. The zoomed images show scanning electron microscopy images of the pointed end and of the bottom of the ring, respectively
image of a ring of about 2 mm outer diameter and a thickness of 25 µm. The rings were electrochemically etched from a thin CoFeSiB foil. The coil wound around the ring is clearly visible in Fig. 4.3b. By choosing the ring orientation, the direction of sensitivity in the surface plane is defined. The outer perimeter of the rings were polished to even out the roughness caused by the etching. After polishing, the perimeter is smooth with some minor polishing traces (see bottom of Fig. 4.3b). Although the rings used as STM electrodes are not sharp, a lateral resolution below 1 nm could be achieved [24, 26]. Most likely nano tips exist at the apex which give a high lateral resolution. To obtain spin contrast, the STM electrodes need to be cleaned in situ by Ar sputtering. The contrast can be increased by coating the CoFeSiB electrodes with several monolayers (ML) of Fe.
4.4 Ferromagnetic Domains and Domain Walls In this section we give several examples on magnetic domains and domain walls in ferromagnets to illustrate the magnetic imaging capabilities of Sp-STM for the in and out-of-plane components of the magnetization. All studies were carried out in ultra high vacuum and at room temperature. The samples were cleaned by Ar ion etching followed by thermal annealing. The sample surfaces were checked for impurities with Auger electron spectroscopy (AES) and no contaminations could be found within the sensitivity limit of our spectrometer. The crystal structure of the surfaces were check with low energy electron diffraction (LEED). All surfaces showed sharp
4 Spin-Polarized Scanning Tunneling Microscopy
129
LEED spots and a low background intensity indicating a single crystalline surface with low concentration of defects. 4.4.1 Ultra-sharp Domain Walls in Co(0001) When using tips that are magnetized perpendicular to the sample plane, the out-ofplane component of the spin polarization may be imaged [21]. While magnetic stray fields of the tip cannot be avoided in this configuration, hard magnetic samples like hcp Co could be imaged without problems. As an example, the closure domain pattern of Co(0001) is presented. Hcp Cobalt has a uniaxial magetocrystalline anisotropy with an easy direction along the c-axis, i.e. perpendicular to the selected (0001) surface. Due to the minimization of the stray field energy, the single domain state is unstable and splits up into a Lifshitz closure domain pattern. Since for Co the magnetic anisotropy and the dipolar energy are of the same order of magnitude, no perfect and simple closure domain structure occurs on the (0001) surface. Instead, the magnetization of most areas of the surface is strongly rotated away from the surface normal and a dendritic pattern is formed [27]. In the MFM image (see Fig. 4.4a), the complex domain pattern of Co(0001) is visible. The limited lateral resolution of MFM becomes apparent at the magnification of the image. In contrast to MFM, Sp-STM reveals the full detail of the fractal structure as depicted in Fig. 4.4b. When zooming into the ends of the fractal branches sharp features in the otherwise smooth contrast can be observed as shown in Fig. 4.5a. The contrast across these sharp features resembles domain walls. The observed contrast corresponds, however, not to a 180◦ domain wall but to an angle of rotation of only 20◦ . The width of the transition region between the two domains is only of the order of 1 nm. At first sight, these small widths seem to contradict common knowledge about domain walls. Bloch walls in bulk Co have a width of ≈ 11 nm. To exclude instrumental reasons for the observation of such sharp walls, we take the following consideration. A mechanism that often causes artificially sharp walls is a magnetostatic pick-up mechanism in which the domain wall is dragged along with the magnetic tip during
Fig. 4.4. (a) MFM and (b) Sp-STM image of the fractal domain pattern of Co(0001). The scans were performed on the same sample but not on the same area
130
W. Wulfhekel · U. Schlickum · J. Kirschner
Fig. 4.5. (a), (b) Sp-STM images of a sharp domain wall on Co(0001). (b) No shift in the wall position is observed when inverting the scan direction excluding dragging of the wall
scanning until it snaps off. In that case, a sharp transition would be observed at the point of snapping off. To test for this mechanism, we recorded the wall while scanning from the right to the left and from the left to the right (see Fig. 4.5b). If the wall was dragged along and snapped off, opposite displacements of the wall for scanning in the two directions should be seen. The domain wall, however, appears at exactly the same position for both directions ruling out any significant dragging. To understand the origin of the specific type of 20◦ wall and to calculate its expected width, we focus on details of the domain pattern of Co(0001). In Co(0001) the magnetocrystalline anisotropy favors a magnetization along the surface normal. To reduce the stray field energy of the sample, domains of opposite magnetization along the normal separated by 180◦ domain walls are formed in the bulk of the crystal. This magnetization configuration reduces the overall stray field, but still produces a large number of surface charges, since the flux is not kept inside the crystal. As Hubert et al. suggested, the system can reduce the amount of surface charges by a partial flux closure with tilted surface domains [28]. From the ratio between magnetocrystalline and dipolar energy one may calculate the angle θ, the magnetization is tilted from the surface normal. Minimizing the free energy results in a large angle of θ ≈ 80◦ [23], i.e. the flux closure is obtained by almost in-plane magnetized surface domains. Hence, one expects to find 20◦ domain walls on the surface in agreement with our Sp-STM observations.
Fig. 4.6. (a) Calculated energy of a 20◦ domain wall in Co(0001) as function of its width. (b) Experimental wall profile (points) and calculated wall profile (solid line) of a 20◦ domain wall
4 Spin-Polarized Scanning Tunneling Microscopy
131
To estimate the width of such a 20◦ domain wall we use a one dimensional model of the domain wall including the magnetic exchange energy and the anisotropy energy of Co [23]. Figure 4.6a shows the wall energy as a function of the wall width w. The minimum energy is found at a wall width of only 1.5 nm. The resulting theoretical wall profile agrees well with the experimentally observed wall profile as depicted in Fig. 4.6b. Especially, the experimental wall profile does not appear blurred when compared to the calculated one indicating a lateral resolution better than 1 nm. The experiments illustrate the possibility, that a domain wall may be narrower than the √ magnetic exchange length of A/K without violation of micromagnetic rules (A and K are the magnetic exchange constant and the magnetic anisotropy, respectively). This holds since the angle of rotation across the wall is small [23]. 4.4.2 Asymmetric Néel Caps in Fe(001) Using ring electrodes, the bottom of the ring is magnetized tangential such that the in-plane component of the spin polarization along the ring plane is imaged [24]. In case the ring is perfect, the magnetic flux is closed and no magnetic stray field exits. This allows the imaging of extremely soft magnetic samples. As an example, the N`eel caps in Fe-whiskers were investigated. Fe-whiskers are needle-like Fe single crystals that are terminated by (001) surfaces. The magnetic ground state is the so called Landau state, in which the flux inside the Fe-whisker is closed. The whisker splits up into two elongated domains that are magnetized along the long side of the whisker. The magnetization at the surface of an Fe-whisker lies in-plane. The domains are separated by a 180◦ domain wall. At the two ends of the whiskers, closure domains are formed. Figure 4.7a shows a magneto optic Kerr effect (MOKE) image of an Fe-whisker taken after sample surface preparation in the UHV chamber. The 180◦ domain wall along 100 can be seen immediately. The MOKE images were recorded to find the position of the wall such that the ring electrode of the Sp-STM can be placed close to the wall.
Fig. 4.7. (a) Magneto optic Kerr image of an Fe-whisker. (b) Topographic and (c) spin signal recorded simultaneously. The 180◦ domain wall seen in (a) is also clearly visible in (c)
132
W. Wulfhekel · U. Schlickum · J. Kirschner
Figure 4.7b,c show the topographic and the magnetic Sp-STM images taken at the same time. In the topographic image, flat terraces of several 100 nm width separated by atomic steps are visible. Fe-whisker surfaces are rather flat which is a necessary condition for imaging with a ring as a dull STM electrode. Nevertheless, the ring electrode allows topographic imaging with nm resolution which can be explained by the existance of nano-tips on the outer ring perimeter. In the image of the spin signal, clearly two domains separated by a 180◦ domain wall running along the 100 direction can be seen. The wall is rather wide. This is not caused by the lateral resolution of the instrument but is due to the magnetic properties of Fe. In the interior of the Fe-whisker, the two domains are separated by a charge free Bloch wall, i.e. the magnetization in the wall rotates in the plane of the wall. At the surface of the whisker, this would lead to an orientation of the wall magnetization perpendicular to the sample surface creating magnetic surface charges. This is energetically unfavorable so that the magnetization of the wall at the surface rotates in the surface plane, i.e. a N´eel cap is formed. As has been shown in detailed calculations, the curling of the Bloch wall to a surface N´eel cap is asymmetric [29] resulting in an asymmetric wall profile at the surface. In Fig. 4.8, the solid line represents the micromagnetically simulated line profile across the 180◦ domain wall. It shows the in-plane component of the magnetization pointing along the domain wall. The measured wall profile (squares) perfectly agrees with the calculated data within the lateral calibration error of the scanner (≈ 10%). The agreement between theory and experiment indicates not only that with Sp-STM one may image a well-defined in-plane component of the spin polarization. It also shows that the ring electrode is indeed free of stray fields. Even small fields of the order of 100 µT are sufficient to move the domain walls in whiskers by several µm. As we see practically no blurring in the experimental wall profile when compared to the theoretical profile, the local stray field of the ring have to be significantly below the above mentioned value.
Fig. 4.8. Calculated (solid ) and measured (squares) wall profile across the N´eel cap on an Fewhisker. The calculations were taken from [29]
4 Spin-Polarized Scanning Tunneling Microscopy
133
4.5 Antiferromagnets in Contact with Ferromagnets Antiferromagnetic surfaces can be investigated as well, as in Sp-STM the spin polarization at the surface is mapped. We here focus on topological antiferromagnets. In these, the magnetic moments within one atomic layer of the crystal couple ferromagnetically while the adjacent layers couple antiferromagentically. In other words: the material is a layered antiferromagnet. We show two examples for these systems which both were grown on Fe(001) as a substrate and both show an in-plane spin polarization. 4.5.1 Mn on Fe(001) and Topologically Induced Frustrations As a model system for the topological antiferromagnets, we focus on Mn grown on Fe(001). Mn can be stabilized at room temperature in a body centered tetragonal (bct) structure on Fe(001) [30]. The bct structure is stable up to about 20 ML [31–33]. Mn films have an out-of-plane lattice constant of 0.323 nm, i.e. a little larger than the 0.287 nm of Fe. Mn grows in a layer-by-layer mode up to 10 to 20 ML [34]. The critical thickness strongly depends on the substrate quality and the growth temperature. When Mn was deposited at room temperature, no intermixing was found. The onset of intermixing was observed by AES for substrate temperatures above 420 K [33, 38]. In STM studies, interdiffusion of Fe into the first ML Mn was found at substrate temperatures above 370 K [39]. The intermixing was observed until the fourth Mn layer [37]. At the Mn surface of films between 4 to 10 ML, small regions with rectangular cross-shaped patterns start to form [36,37]. It was speculated that these small rectangular islands are local reconstructions and a precursor to threedimensional growth. The first evidence that Mn on Fe(001) is a layer-wise antiferromagnet was reported by Walker and Hopster [38]. This was confirmed with scanning electron microscopy with polarization analysis (SEMPA) [34] and later with spin-polarized STM in the spectroscopic mode [20].
Fig. 4.9. (a) Topographic STM image and (b) line scan of 7 ML Mn on Fe(001). (c) Magnetic Sp-STM image of the same area and (d) line scan revealing the layer-wise antiferromagnetic order of bct Mn. The direction of sensitivity for the spin is parallel to the whisker axis and is indicated in (c)
134
W. Wulfhekel · U. Schlickum · J. Kirschner
Figure 4.9 shows the example of a thin Mn film grown on Fe(001). The topographic image of the Mn film indicates an imperfect layer-by-layer growth as several layers are exposed at the surface. The terraces are separated by single atomic steps as can be deduced from the line scan in Fig. 4.9b. The Fe substrate was homogenously magnetized in one direction over the whole imaged area, as determined by Kerr-microscopy. The direction of sensitivity of the ring was chosen collinear to the magnetization of the Fe substrate. Thus, the imaged spin signal shows the projection of the spin component collinear to the Fe magnetization. The Sp-STM images taken simultaneously to the topographic images show an alternating contrast on the atomic terraces of Mn (see Fig. 4.9c) confirming a layer-wise antiferromagnetic order. In agreement to that, the spin signal is identical on all terraces but the sign alters (see the line scan in Fig. 4.9d). This ideal antiferromagnetic order was found on most areas of the Mn film. The unperturbed layer-wise antiferromagnetic order is, however, disturbed in case a step of the underlaying Fe substrate is present. Figure 4.10a presents schematically the topological and magnetic situation of Mn layers overgrowing a step edge of the Fe substrate underneath. The thickness of the Mn layers on both sides of a monatomic Fe step differs by one ML. Due to the vertical lattice mismatch, subatomic steps are formed at the Mn film surface at the position of Fe step edges. The situation of the magnetic order above such step edges is more complicated. An undisturbed layer-wise antiferromagnetic order within the Mn film is not possible when the Mn moments at the interface on both sides of the step edge are aligned in the same direction by the Fe substrate. Instead, Mn layers which meet at the position of the Fe step edge are magnetized oppositely. This leads to a magnetic frustration [40, 41]. Figure 4.10b shows a Sp-STM image of the topography of a Mn film grown over a monatomic step of the Fe substrate. In the topography, a buried Fe step edge is running almost vertically through the center of the imaged area (black arrows as guideline). The line profile in Fig. 4.10c taken along the black line in Fig. 4.10b shows a step of monatomic height between two different Mn terraces (≈ 0.16 nm) and a step of subatomic height (≈ 0.018 nm) at the position of a buried Fe step edge due to the different lattice constants of Fe and Mn. In Fig. 4.10d clearly the layer-wise antiferromagnetic order between the Mn islands and the Mn layer underneath is visible. Following the way of the buried Fe step edge, a magnetically frustrated region is present. Along the buried Fe step edge, a reversal of the spin contrast appears. In this region the spin polarization of the Mn rotates by 180◦ . The observation of magnetically frustrated regions at the surface of thin Mn films at the position of buried Fe step edges indicates that the magnetic frustrations are extended throughout the whole Mn film down to the interface, as schematically shown in Fig. 4.10a. This implies that the coupling energy at the interface between Fe and Mn is higher than the domain wall energy in the Mn film which is likely for thin films. Figure 4.10e presents an averaged line profile across the topologically enforced magnetic frustration at the position of the box in Fig. 4.10d. The measurement indicates that the magnetic frustration has a certain lateral extension. To estimate the wall width at the surface, the experimental profil